Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3897_Position 118_00000.hld	2733.748462	556823.653898	529.505813	187554203.993819	3527.854081	3522.441862	34.256435	2.968868	15.715796	2016.916680	1.431664	-130.587000	-59.581000	0.046883
3897_Position 118_00001.hld	2695.767513	567710.004844	515.083135	182454574.665871	3525.000169	3522.396216	33.785845	3.111514	17.780006	1967.050198	1.411165	-130.537000	-59.580500	0.047683
3897_Position 118_00002.hld	2687.927161	568005.396877	511.332066	181410649.771486	3524.969608	3521.053179	33.636164	3.131048	20.407120	1973.213797	1.393402	-130.487000	-59.581000	0.014797
3897_Position 118_00003.hld	2666.966124	577134.322336	506.710823	178634496.460945	3524.013310	3521.202352	33.590181	3.230811	18.474522	1923.183308	1.403024	-130.437000	-59.581000	0.003798
3897_Position 118_00004.hld	2685.505647	570616.425263	512.368693	181088838.312559	3524.434881	3520.768075	33.734290	3.151030	25.005937	1995.966992	1.369152	-130.387000	-59.581000	0.033434
3897_Position 118_00005.hld	2664.094287	576108.189263	503.461029	178255813.708812	3524.289947	3522.315912	33.410182	3.231918	27.340089	1971.603847	1.355167	-130.587000	-59.531000	0.006889
3897_Position 118_00006.hld	2663.752474	572639.781183	500.278853	178210768.871222	3524.411066	3522.233366	33.203205	3.213273	24.222226	1955.341703	1.368893	-130.537000	-59.531000	-0.035282
3897_Position 118_00007.hld	2649.499302	575622.066608	494.663666	176337540.323628	3523.292962	3522.246947	33.004446	3.264319	24.216536	1931.696927	1.366847	-130.487000	-59.531000	0.045854
3897_Position 118_00008.hld	2672.131342	570316.678068	503.682763	179316601.111710	3524.730445	3521.351406	33.325883	3.180501	25.843754	1978.692936	1.362419	-130.437000	-59.531000	0.072738
3897_Position 118_00009.hld	2675.345822	568274.440246	503.484887	179741755.262637	3524.950118	3521.857488	33.273369	3.161616	28.976790	1999.514035	1.348780	-130.387000	-59.531000	-0.006799
3897_Position 118_00010.hld	2661.959746	573749.528827	499.712286	177974612.781351	3524.603231	3523.079553	33.187598	3.223772	24.378442	1952.565452	1.367853	-130.587000	-59.481000	0.062892
3897_Position 118_00011.hld	2677.565884	554990.926311	493.467482	180035680.591876	3523.611555	3521.072721	32.584726	3.082672	23.991115	1981.191997	1.369177	-130.537000	-59.481000	0.121929
3897_Position 118_00012.hld	2673.999016	562936.631364	498.521839	179563562.277615	3523.570109	3520.907697	32.961723	3.135027	26.914752	1989.209581	1.356431	-130.487000	-59.481000	0.097018
3897_Position 118_00013.hld	2664.335599	569141.155163	498.211921	178287617.839671	3523.596906	3521.111297	33.058896	3.192264	32.215309	1996.849711	1.334300	-130.437000	-59.481000	0.042385
3897_Position 118_00014.hld	2639.327737	589064.505072	501.240499	175006812.753755	3524.575073	3520.737719	33.570167	3.365952	29.083702	1938.757826	1.346121	-130.387000	-59.481000	0.157060
3897_Position 118_00015.hld	2664.132526	563959.004905	493.903805	178260853.341733	3524.092288	3520.512351	32.775491	3.163673	33.789000	2004.665415	1.327548	-130.587000	-59.431000	0.135791
3897_Position 118_00016.hld	2653.270241	573866.150244	496.728176	176832170.945817	3524.453913	3519.739335	33.095808	3.245259	31.165570	1974.578433	1.337463	-130.537000	-59.431000	0.170832
3897_Position 118_00017.hld	2663.557222	569868.259896	499.690020	178185040.680778	3524.266055	3518.889884	33.166518	3.198182	35.680543	2010.711015	1.322449	-130.487000	-59.431000	0.040841
3897_Position 118_00018.hld	2653.209121	579341.569793	502.366373	176824148.378618	3523.705515	3518.128034	33.472227	3.276371	30.686972	1971.948418	1.340744	-130.437000	-59.431000	0.156217
3897_Position 118_00019.hld	2658.035226	576346.736960	503.029869	177458184.136826	3523.487494	3517.348121	33.456506	3.247789	31.860483	1985.862578	1.336666	-130.387000	-59.431000	0.113669
3897_Position 118_00020.hld	2663.364792	562184.134908	493.749152	178159686.118560	3524.032204	3517.316844	32.774530	3.155507	38.467373	2023.439604	1.312027	-130.587000	-59.381000	0.034916
3897_Position 118_00021.hld	2666.621494	564263.827166	497.794673	178589031.963677	3524.108035	3516.766932	33.003324	3.159566	39.913011	2033.280847	1.308734	-130.537000	-59.381000	0.115682
3897_Position 118_00022.hld	2647.022471	580262.796157	500.486529	176013034.954492	3523.432319	3516.570545	33.423722	3.296704	39.420786	1997.718324	1.310036	-130.487000	-59.381000	0.115888
3897_Position 118_00023.hld	2659.164598	574672.313961	502.903368	177606721.313879	3523.559908	3516.196511	33.434103	3.235645	41.588674	2025.288057	1.304714	-130.437000	-59.381000	0.118285
3897_Position 118_00024.hld	2656.660627	576315.618772	502.944096	177277478.437121	3522.675439	3516.073665	33.467846	3.250924	41.112170	2019.539420	1.306008	-130.387000	-59.381000	0.113208