Thu Aug 25 12:16:03 2022

Number of Points = 9926

Depth (nm)	Load (N)	Time (s)
2.302016	105.342277	0.000000
1.817416	100.141031	0.005005
2.080695	87.087241	0.010010
1.701159	89.652360	0.015014
1.631979	79.286069	0.020019
1.320924	74.854904	0.025024
1.175770	71.606296	0.030029
0.997060	49.896177	0.035034
0.759276	56.912612	0.040038
0.821340	48.908074	0.045043
0.211718	36.506779	0.050048
0.004235	40.898885	0.055053
-0.214540	23.912211	0.060058
-0.371374	32.687647	0.065062
-1.467223	26.000326	0.070067
-2.149581	21.959544	0.075072
-2.719876	31.897578	0.080077
-2.436997	20.172700	0.085082
-2.191399	25.034810	0.090086
-2.250443	27.024525	0.095091
-2.374723	15.619707	0.100096
-3.002160	23.896237	0.105101
-3.804140	24.752680	0.110106
-3.794365	26.981547	0.115110
-4.083820	16.162591	0.120115
-4.146528	18.421795	0.125120
-4.266278	26.305571	0.130125
-4.190898	23.968377	0.135130
-4.576254	22.687294	0.140134
-5.467646	23.753898	0.145139
-5.041552	24.443233	0.150144
-5.602519	27.081063	0.155149
-5.616666	17.791347	0.160154
-6.386278	13.403572	0.165158
-6.905719	17.711674	0.170163
-6.443356	13.134033	0.175168
-6.702480	21.669228	0.180173
-6.811451	15.377775	0.185178
-7.263428	26.056564	0.190182
-7.875774	25.465940	0.195187
-8.081058	14.459792	0.200192
-8.487855	20.351095	0.205197
-8.127908	15.770518	0.210202
-8.552601	16.915858	0.215206
-8.496429	12.775181	0.220211
-9.241971	8.617753	0.225216
-9.757436	15.791575	0.230221
-9.694805	9.856049	0.235226
-9.903358	21.863428	0.240230
-10.015327	11.197000	0.245235
-9.612433	9.384291	0.250240
-10.884833	17.382225	0.255245
-10.871638	10.309173	0.260250
-11.640111	12.780198	0.265254
-11.668401	10.917990	0.270259
-11.442243	10.996413	0.275264
-11.977935	21.950906	0.280269
-12.247159	15.937661	0.285274
-12.771310	14.615052	0.290278
-13.376859	21.110132	0.295283
-13.045410	16.926324	0.300288
-13.015672	12.811935	0.305293
-12.958185	14.489162	0.310298
-12.976964	12.752013	0.315302
-13.579941	21.591019	0.320307
-14.122132	20.312364	0.325312
-14.496486	23.699234	0.330317
-14.238754	20.947492	0.335322
-14.895586	13.862363	0.340326
-15.639903	24.953949	0.345331
-15.620722	13.396943	0.350336
-15.724056	21.404693	0.355341
-15.757582	19.106710	0.360346
-16.025501	26.646707	0.365350
-16.083195	23.485646	0.370355
-16.828078	15.395589	0.375360
-16.942838	26.363225	0.380365
-17.377923	17.528605	0.385370
-17.260171	16.323717	0.390374
-17.341710	17.108408	0.395379
-17.365054	20.759816	0.400384
-18.278307	23.313639	0.405389
-18.384114	20.549256	0.410394
-18.510345	15.314033	0.415398
-18.777282	11.590976	0.420403
-19.312450	14.477861	0.425408
-19.868926	17.738242	0.430413
-19.884893	16.475213	0.435418
-19.502820	24.925762	0.440422
-19.883800	22.868879	0.445427
-20.048948	23.812202	0.450432
-20.804520	31.890515	0.455437
-21.007279	16.505358	0.460442
-20.539780	17.738694	0.465446
-20.914588	28.047890	0.470451
-21.462356	20.746355	0.475456
-22.416262	30.741330	0.480461
-22.339325	22.282061	0.485466
-22.432279	19.911131	0.490470
-22.533862	12.875045	0.495475
-22.920575	10.104058	0.500480
-23.403064	23.913395	0.505485
-23.404883	16.921787	0.510490
-23.438171	17.252831	0.515494
-23.750007	19.490959	0.520499
-24.071172	15.042412	0.525504
-24.875102	14.307803	0.530509
-24.934629	16.209007	0.535514
-25.222744	14.966474	0.540518
-25.241772	18.756409	0.545523
-24.987426	22.535150	0.550528
-25.441330	17.044385	0.555533
-26.068103	22.539888	0.560538
-26.657977	19.800732	0.565542
-27.045276	27.096845	0.570547
-26.809878	18.925958	0.575552
-27.204871	25.780353	0.580557
-26.780396	23.192309	0.585562
-26.887169	27.609760	0.590566
-27.566392	23.577980	0.595571
-27.964306	12.000908	0.600576
-28.370713	18.800141	0.605581
-28.092185	17.734576	0.610586
-28.540483	16.555106	0.615590
-28.881487	16.719230	0.620595
-29.235873	16.271687	0.625600
-29.693814	24.331836	0.630605
-29.792466	26.840281	0.635610
-29.880533	21.013785	0.640614
-30.055145	27.425528	0.645619
-30.035905	18.421647	0.650624
-31.056977	25.513343	0.655629
-31.286241	25.621995	0.660634
-31.281510	17.401831	0.665638
-31.434251	14.084823	0.670643
-31.437266	12.908349	0.675648
-31.882710	21.972606	0.680653
-32.340884	14.574780	0.685658
-32.400520	11.777855	0.690662
-32.772316	19.425873	0.695667
-32.502503	12.461308	0.700672
-32.990010	15.714047	0.705677
-33.615635	21.636473	0.710682
-33.908144	17.338460	0.715686
-34.684916	15.739061	0.720691
-34.360122	16.339863	0.725696
-34.671557	23.374152	0.730701
-34.499010	22.603601	0.735706
-34.340354	23.629066	0.740710
-35.046781	16.950340	0.745715
-35.447256	10.954500	0.750720
-35.432389	20.535087	0.755725
-35.827741	18.410855	0.760730
-36.292082	21.014563	0.765734
-37.221495	26.127218	0.770739
-36.931423	16.811985	0.775744
-37.117377	22.178306	0.780749
-37.299029	13.167941	0.785754
-37.139416	15.803596	0.790758
-37.143744	17.999869	0.795763
-37.487240	10.881467	0.800768
-38.697350	13.700102	0.805773
-38.684821	12.983098	0.810778
-38.711908	15.141808	0.815782
-38.993542	18.197776	0.820787
-38.548206	11.265820	0.825792
-39.466794	18.705286	0.830797
-39.960603	14.600165	0.835802
-40.319998	23.891385	0.840806
-40.476259	15.329454	0.845811
-40.155677	20.163993	0.850816
-40.344644	21.832380	0.855821
-40.527111	21.516086	0.860826
-41.092248	21.259752	0.865830
-41.478217	9.057556	0.870835
-41.250284	10.647964	0.875840
-42.446855	16.593411	0.880845
-42.559485	11.352896	0.885850
-42.523709	17.291910	0.890854
-42.763496	16.658733	0.895859
-42.953867	16.220293	0.900864
-43.197932	11.417984	0.905869
-43.567961	7.445330	0.910874
-43.631405	21.682547	0.915878
-44.350425	24.218594	0.920883
-44.216134	11.181910	0.925888
-44.445057	24.970498	0.930893
-44.316670	29.303647	0.935898
-44.491900	16.018066	0.940902
-45.273594	15.257829	0.945907
-45.462686	14.085201	0.950912
-45.654120	17.275731	0.955917
-46.026918	14.894867	0.960922
-46.658735	16.496602	0.965926
-47.142445	22.387302	0.970931
-46.831189	16.444457	0.975936
-47.348645	20.103683	0.980941
-47.158961	12.734061	0.985946
-46.939424	12.601550	0.990950
-47.544986	24.152281	0.995955
-47.373650	29.310763	1.000960
-48.016225	20.676334	1.005965
-47.951238	20.378215	1.010970
-48.773142	16.441561	1.015974
-49.595242	19.534757	1.020979
-49.764371	21.753689	1.025984
-50.214026	20.397263	1.030989
-49.508899	22.314696	1.035994
-50.084869	21.857580	1.040998
-50.194388	20.457351	1.046003
-49.971922	22.909152	1.051008
-50.524260	23.631571	1.056013
-51.106232	22.779929	1.061018
-51.181420	13.135955	1.066022
-51.498309	18.620867	1.071027
-51.421203	24.986839	1.076032
-51.890163	24.927406	1.081037
-52.448335	21.503081	1.086042
-52.761719	13.459315	1.091046
-53.297088	17.580089	1.096051
-53.002744	20.738796	1.101056
-53.116145	28.067921	1.106061
-53.132752	18.145848	1.111066
-53.159958	17.979232	1.116070
-53.974464	21.106040	1.121075
-54.206236	22.328720	1.126080
-54.470786	21.205881	1.131085
-54.510110	13.837340	1.136090
-55.050276	16.440273	1.141094
-55.834334	12.583112	1.146099
-55.810184	18.884614	1.151104
-55.851422	14.275150	1.156109
-55.676638	15.516384	1.161114
-55.646890	13.189505	1.166118
-56.422176	17.028335	1.171123
-56.935029	19.127119	1.176128
-57.239254	21.117284	1.181133
-57.195992	23.306101	1.186138
-57.115779	17.250762	1.191142
-58.123891	21.062799	1.196147
-58.549507	23.742697	1.201152
-58.917370	24.160966	1.206157
-58.852037	19.420908	1.211162
-58.910126	11.621878	1.216166
-58.850860	13.988518	1.221171
-59.001113	11.300705	1.226176
-58.795936	22.218204	1.231181
-59.262411	15.087435	1.236186
-59.995687	16.524735	1.241190
-60.612652	13.644296	1.246195
-60.375924	14.281042	1.251200
-60.631274	14.662699	1.256205
-61.098691	11.562677	1.261210
-61.544411	12.977067	1.266214
-62.219300	10.042430	1.271219
-62.001123	13.557916	1.276224
-62.221564	11.172164	1.281229
-62.190726	5.273261	1.286234
-61.983848	4.440385	1.291238
-62.270016	10.752542	1.296243
-63.104597	9.519706	1.301248
-63.303864	20.177875	1.306253
-63.467338	17.954037	1.311258
-63.338201	12.742078	1.316262
-64.109836	18.323554	1.321267
-64.628915	11.637625	1.326272
-64.845984	16.521604	1.331277
-64.996947	14.514104	1.336282
-65.317491	10.888035	1.341286
-65.188022	25.003277	1.346291
-65.074517	14.162319	1.351296
-65.708547	22.882805	1.356301
-66.202223	11.804795	1.361306
-66.736230	10.284419	1.366310
-66.811513	16.136431	1.371315
-66.633357	14.248203	1.376320
-66.682457	21.197093	1.381325
-66.971792	21.346795	1.386330
-67.084086	17.495106	1.391334
-67.884631	22.011771	1.396339
-67.606876	16.279818	1.401344
-68.090912	29.238354	1.406349
-68.789203	17.872865	1.411354
-68.878912	22.531247	1.416358
-69.105141	33.342343	1.421363
-69.430513	33.611587	1.426368
-68.947303	31.732506	1.431373
-69.946629	22.483267	1.436378
-70.163347	16.518747	1.441382
-70.629591	30.366670	1.446387
-70.407228	23.352590	1.451392
-70.626963	24.279157	1.456397
-70.809971	24.355251	1.461402
-71.108624	16.207938	1.466406
-71.711230	23.604223	1.471411
-71.554535	19.185206	1.476416
-71.778755	21.599431	1.481421
-72.649603	22.412887	1.486426
-72.990607	21.134350	1.491430
-73.208047	28.169731	1.496435
-73.477269	24.466015	1.501440
-73.606881	22.540591	1.506445
-73.604450	21.594216	1.511450
-73.376540	22.083648	1.516454
-73.660578	27.057217	1.521459
-73.653298	21.437246	1.526464
-74.853107	22.185189	1.531469
-74.962976	25.574910	1.536474
-75.371665	23.667904	1.541478
-75.376962	20.213898	1.546483
-75.103811	12.119359	1.551488
-75.912299	21.898557	1.556493
-76.709158	17.192359	1.561498
-76.283222	14.028286	1.566502
-76.371956	20.271545	1.571507
-76.511538	11.558311	1.576512
-76.556475	12.005075	1.581517
-77.316338	17.138619	1.586522
-77.287872	6.355284	1.591526
-77.751935	13.416647	1.596531
-77.831263	9.404772	1.601536
-78.178166	16.732514	1.606541
-78.965468	13.461155	1.611546
-78.916705	13.513589	1.616550
-79.288118	15.871783	1.621555
-79.035865	8.932119	1.626560
-79.118678	5.797145	1.631565
-80.065086	9.286303	1.636570
-80.375691	13.738852	1.641574
-80.484428	16.796201	1.646579
-80.616482	8.110263	1.651584
-80.821099	5.661922	1.656589
-80.936475	8.204622	1.661594
-80.991570	9.295214	1.666598
-81.978241	12.072515	1.671603
-81.945777	3.661355	1.676608
-82.139208	7.285627	1.681613
-82.119141	7.845590	1.686618
-81.993735	9.961422	1.691622
-83.440299	18.382119	1.696627
-83.517328	17.046402	1.701632
-83.855880	13.575014	1.706637
-83.934629	13.005190	1.711642
-83.708984	6.667642	1.716646
-84.004512	11.557586	1.721651
-83.569983	-0.380859	1.726656
-83.976574	7.880041	1.731661
-84.810942	4.916614	1.736666
-85.162928	7.575482	1.741670
-85.411484	6.839277	1.746675
-85.137934	5.723872	1.751680
-85.837209	12.277929	1.756685
-86.433584	9.764424	1.761690
-86.563465	8.500263	1.766694
-86.957947	13.405713	1.771699
-86.932180	5.985850	1.776704
-86.446630	3.508460	1.781709
-87.144285	5.228079	1.786714
-87.806777	6.442320	1.791718
-88.090932	14.794769	1.796723
-88.201329	2.897416	1.801728
-88.431856	12.298147	1.806733
-88.430173	10.174982	1.811738
-88.635395	6.173344	1.816742
-89.127110	10.859913	1.821747
-89.521447	13.452652	1.826752
-89.549047	12.159809	1.831757
-89.754701	8.382863	1.836762
-89.544435	8.198020	1.841766
-90.385131	7.355285	1.846771
-90.524690	8.987456	1.851776
-91.000654	-1.137870	1.856781
-91.050758	0.774510	1.861786
-90.978448	5.363207	1.866790
-91.725259	15.835086	1.871795
-92.189015	5.461073	1.876800
-92.518844	5.743670	1.881805
-92.637883	9.425887	1.886810
-92.614915	9.422252	1.891814
-92.532568	20.450740	1.896819
-92.550060	13.376173	1.901824
-93.378865	22.348639	1.906829
-93.708961	16.006420	1.911834
-93.811795	15.611212	1.916838
-94.314201	11.342930	1.921843
-94.020029	5.630554	1.926848
-94.452725	13.117270	1.931853
-95.339977	11.987603	1.936858
-95.174264	9.914665	1.941862
-95.341040	5.691869	1.946867
-95.773656	12.704012	1.951872
-95.519984	17.102944	1.956877
-95.890088	9.318007	1.961882
-96.296934	9.052692	1.966886
-96.735474	11.453042	1.971891
-96.941667	11.871290	1.976896
-96.732879	15.802694	1.981901
-97.142020	9.548793	1.986906
-97.834542	3.219077	1.991910
-98.442591	20.600951	1.996915
-98.521336	18.055944	2.006912
-97.474713	17.283657	2.016909
-97.285247	14.542272	2.026906
-97.200110	12.571168	2.036902
-96.446176	13.780259	2.046899
-95.883294	15.899931	2.056896
-95.561108	14.056408	2.066893
-94.966734	18.176353	2.076890
-94.755729	14.110627	2.086886
-93.442375	16.448490	2.096883
-93.399973	16.669853	2.106880
-93.093019	15.218354	2.116877
-92.260230	10.117536	2.126874
-91.754613	12.784704	2.136870
-91.739712	13.409517	2.146867
-90.920822	15.780511	2.156864
-90.491414	14.148267	2.166861
-89.486296	12.653894	2.176858
-89.416830	16.875095	2.186854
-89.239417	11.493668	2.196851
-88.516022	13.464645	2.206848
-87.914820	13.715657	2.216845
-86.927810	8.210540	2.226842
-86.665613	14.612654	2.236838
-86.518108	16.167024	2.246835
-86.053777	11.082759	2.256832
-85.312663	12.113297	2.266829
-84.913064	11.565939	2.276826
-84.240487	10.187029	2.286822
-83.411562	8.932506	2.296819
-83.459352	8.189157	2.306816
-83.221941	14.284712	2.316813
-82.402876	12.632593	2.326810
-82.006996	20.927105	2.336806
-80.860002	17.756918	2.346803
-80.592288	18.709580	2.356800
-80.728030	13.906240	2.366797
-80.032132	19.657527	2.376794
-79.131788	18.417156	2.386790
-78.912648	16.101940	2.396787
-78.467749	17.052182	2.406784
-77.880533	11.292931	2.416781
-77.637234	19.009471	2.426778
-76.868823	20.647115	2.436774
-76.541086	17.082614	2.446771
-75.798165	16.928118	2.456768
-75.163171	19.907634	2.466765
-75.002156	14.693499	2.476762
-74.161431	16.791812	2.486758
-73.647485	11.889840	2.496755
-73.694046	9.755641	2.506752
-72.509595	13.995369	2.516749
-72.208406	11.936559	2.526746
-71.973145	13.046360	2.536742
-71.479666	19.006761	2.546739
-70.883180	16.271291	2.556736
-70.465998	13.915541	2.566733
-69.562940	16.010423	2.576730
-69.520600	17.970910	2.586726
-69.226629	10.230226	2.596723
-68.330736	14.996672	2.606720
-67.551117	10.354012	2.616717
-66.971631	15.090842	2.626714
-66.862660	10.233320	2.636710
-66.636925	13.064721	2.646707
-65.876932	5.396735	2.656704
-65.645604	9.785809	2.666701
-64.857858	10.432075	2.676698
-64.267403	16.909468	2.686694
-63.806485	17.689308	2.696691
-63.304221	21.538589	2.706688
-63.144705	19.558998	2.716685
-61.919387	24.102770	2.726682
-61.466677	19.254740	2.736678
-61.261846	14.334679	2.746675
-61.299703	14.378551	2.756672
-59.988079	16.038785	2.766669
-60.130149	22.897054	2.776666
-59.103594	12.792453	2.786662
-58.494958	16.884824	2.796659
-58.435595	12.535584	2.806656
-58.277741	21.488280	2.816653
-57.347927	23.936932	2.826650
-56.510627	19.123675	2.836646
-55.814038	21.529676	2.846643
-55.474738	18.359337	2.856640
-55.680672	22.313250	2.866637
-55.529177	24.288312	2.876634
-54.254169	23.562607	2.886630
-53.455091	24.660093	2.896627
-52.933032	14.029492	2.906624
-52.808973	18.308665	2.916621
-52.879662	21.481118	2.926618
-51.950414	21.474824	2.936614
-51.039557	14.571976	2.946611
-50.379513	10.768509	2.956608
-49.937727	23.218301	2.966605
-49.667141	14.233171	2.976602
-49.542470	14.508167	2.986598
-48.913545	17.380931	2.996595
-48.143390	17.263352	3.006592
-47.955499	27.621010	3.016589
-47.127798	17.997389	3.026586
-46.841621	24.842411	3.036582
-46.440158	16.340451	3.046579
-45.477516	16.531664	3.056576
-45.382053	14.086941	3.066573
-45.097930	14.444658	3.076570
-44.210859	21.772063	3.086566
-43.869149	17.251870	3.096563
-43.042269	17.977537	3.106560
-43.012682	17.614868	3.116557
-42.333763	19.805061	3.126554
-41.391906	15.029276	3.136550
-41.117950	16.031646	3.146547
-40.939208	17.932748	3.156544
-39.823889	21.001732	3.166541
-39.722511	21.080807	3.176538
-39.639695	19.094227	3.186534
-38.706767	14.747492	3.196531
-38.296839	14.407591	3.206528
-37.707658	13.212811	3.216525
-36.986276	15.751143	3.226522
-37.018319	14.115178	3.236518
-36.099435	7.901652	3.246515
-35.227848	10.194703	3.256512
-34.907562	12.358727	3.266509
-35.015105	17.374270	3.276506
-34.684140	16.600083	3.286502
-33.732577	14.119423	3.296499
-33.370744	11.686816	3.306496
-32.574923	11.872492	3.316493
-32.312339	11.549342	3.326490
-31.698989	16.559636	3.336486
-30.951198	16.657803	3.346483
-30.976099	15.619430	3.356480
-30.351077	18.819090	3.366477
-29.633725	18.766806	3.376474
-29.338010	19.547190	3.386470
-28.701421	14.724203	3.396467
-27.713564	14.673884	3.406464
-27.801725	10.154523	3.416461
-27.686224	16.481427	3.426458
-26.708581	16.204627	3.436454
-26.065035	13.974967	3.446451
-25.340083	19.208528	3.456448
-25.224266	15.483998	3.466445
-25.167547	13.124540	3.476442
-24.088857	13.497143	3.486438
-23.624356	5.058170	3.496435
-23.231822	4.017747	3.506432
-22.840773	8.410307	3.516429
-22.472864	14.000749	3.526426
-21.696648	7.331242	3.536422
-21.077023	15.175721	3.546419
-21.030512	9.672252	3.556416
-20.117649	14.261818	3.566413
-19.757588	11.892845	3.576410
-19.137572	17.681371	3.586406
-18.066436	10.420795	3.596403
-18.062489	15.298493	3.606400
-18.054025	15.959161	3.616397
-17.339442	16.182909	3.626394
-16.821498	10.339479	3.636390
-16.312839	17.608970	3.646387
-15.104179	13.668860	3.656384
-15.127934	13.441260	3.666381
-15.031390	14.968772	3.676378
-14.110988	22.639416	3.686374
-13.670528	21.312718	3.696371
-13.383975	15.087395	3.706368
-12.168600	18.745753	3.716365
-11.948582	14.187607	3.726362
-12.298257	17.869437	3.736358
-11.203617	17.548966	3.746355
-10.746016	14.512145	3.756352
-9.953678	17.891498	3.766349
-9.507887	17.916610	3.776346
-9.188996	5.394999	3.786342
-8.940347	10.623993	3.796339
-8.167288	14.665265	3.806336
-7.984910	17.493959	3.816333
-6.890698	21.507088	3.826330
-6.472576	21.514361	3.836326
-6.466776	16.045779	3.846323
-5.447273	21.160332	3.856320
-5.175807	21.035362	3.866317
-4.855755	22.163559	3.876314
-3.974745	26.783464	3.886310
-3.809011	24.783891	3.896307
-3.352084	27.842000	3.906304
-2.598188	29.662491	3.916301
-2.515660	40.385127	3.926298
-1.857409	59.678312	3.936294
-1.756371	62.405718	3.946291
-1.321390	75.952679	3.956288
-0.763449	95.375660	3.966285
-0.233763	114.765076	3.976282
0.000000	127.377067	3.981286
0.004180	137.481413	3.986291
0.345228	147.090058	3.991296
0.476622	153.064759	3.996301
0.932863	157.669275	4.001306
0.650742	160.298235	4.006310
0.701965	164.241711	4.011315
1.079173	161.433263	4.016320
1.206936	169.110642	4.021325
1.423491	156.016666	4.026330
0.980441	168.374098	4.031334
0.882418	165.314242	4.036339
0.888573	157.669593	4.041344
1.052277	184.599170	4.046349
0.999890	181.082907	4.051354
1.336789	189.901284	4.056358
1.348127	194.246487	4.061363
1.391991	190.980897	4.066368
1.294636	189.151638	4.071373
1.350250	183.138060	4.076378
1.332284	191.645041	4.081382
1.196701	187.116752	4.086387
1.508938	184.932251	4.091392
1.198894	196.553852	4.096397
1.464497	194.041297	4.101402
1.442058	187.426176	4.106406
1.082716	182.869671	4.111411
1.404880	190.459652	4.116416
1.388191	188.070423	4.121421
1.446573	187.001377	4.126426
1.198685	188.552460	4.131430
1.357103	193.750981	4.136435
1.268781	184.124786	4.141440
1.283771	191.433865	4.146445
1.592925	189.531422	4.151450
1.398957	194.272625	4.156454
1.629278	200.712735	4.161459
1.834470	190.341355	4.166464
1.444676	201.548346	4.171469
1.495856	187.607058	4.176474
1.692254	194.289762	4.181478
1.720416	183.920814	4.186483
1.980358	189.201504	4.191488
1.264427	197.083853	4.196493
1.585863	186.555056	4.201498
1.735000	186.996726	4.206502
1.798336	195.702944	4.211507
1.597712	181.987776	4.216512
1.369450	191.457854	4.221517
1.899910	201.444977	4.226522
1.806191	197.156899	4.231526
1.772169	203.546678	4.236531
1.635819	198.306658	4.241536
1.635114	194.434279	4.246541
1.782611	189.383907	4.251546
1.665282	190.920861	4.256550
1.856365	185.664343	4.261555
1.672147	189.837704	4.266560
1.545630	195.308661	4.271565
1.764835	188.253880	4.276570
1.899675	188.621859	4.281574
1.711971	197.841976	4.286579
1.708493	185.503793	4.291584
1.530182	194.336457	4.296589
1.633032	192.899774	4.301594
1.215182	190.263350	4.306598
1.372851	196.638910	4.311603
1.855651	202.466819	4.316608
2.043324	215.690411	4.321613
2.030168	207.944361	4.326618
1.782143	207.628843	4.331622
2.102015	222.264914	4.336627
2.059996	205.819852	4.341632
1.607614	201.325376	4.346637
2.103699	215.136562	4.351642
2.108098	216.031183	4.356646
1.825870	218.014758	4.361651
1.814682	220.345010	4.366656
1.681622	223.501120	4.371661
1.952563	218.763594	4.376666
1.576467	223.432101	4.381670
1.956317	227.539237	4.386675
2.184288	219.853479	4.391680
1.984094	229.771600	4.396685
2.036950	224.565202	4.401690
2.169025	216.774247	4.406694
2.004195	223.032667	4.411699
2.280455	218.889096	4.416704
2.079846	225.358768	4.421709
2.325623	220.568236	4.426714
2.172672	225.211272	4.431718
1.997515	223.242339	4.436723
2.407505	223.013547	4.441728
1.917394	232.578459	4.446733
2.420272	218.791002	4.451738
2.216177	226.026853	4.456742
1.837725	226.421473	4.461747
2.130790	216.586806	4.466752
2.222033	221.144124	4.471757
2.080821	221.242143	4.476762
2.147298	228.479894	4.481766
2.230892	243.308027	4.486771
2.483356	239.370662	4.491776
2.168760	251.856723	4.496781
2.539801	247.378754	4.501786
2.438597	248.112751	4.506790
2.526228	244.919389	4.511795
2.573719	233.971575	4.516800
2.288911	230.738493	4.521805
2.446522	221.399613	4.526810
2.090122	223.255604	4.531814
2.422113	242.429807	4.536819
2.950383	245.786025	4.541824
2.404455	236.054329	4.546829
2.461930	231.986164	4.551834
2.379958	230.091215	4.556838
2.485892	239.388733	4.561843
2.293000	238.017366	4.566848
2.485230	243.625059	4.571853
2.765158	246.909455	4.576858
2.768047	248.898982	4.581862
2.493643	243.041496	4.586867
2.410203	226.644033	4.591872
2.350937	248.223901	4.596877
2.483099	255.660181	4.601882
2.739658	250.595867	4.606886
2.656179	252.247746	4.611891
2.929245	250.430046	4.616896
2.877243	256.730911	4.621901
2.987197	248.041732	4.626906
2.196522	233.722943	4.631910
2.062065	247.265951	4.636915
2.845960	248.854695	4.641920
2.500065	255.799562	4.646925
2.613260	249.185313	4.651930
2.645268	253.052725	4.656934
2.428479	258.613776	4.661939
2.434476	249.573885	4.666944
2.237269	256.084164	4.671949
2.693887	255.341863	4.676954
2.379529	264.249662	4.681958
2.932944	285.132460	4.686963
2.683162	284.048416	4.691968
2.602642	288.768706	4.696973
2.754812	278.867495	4.701978
2.659284	284.400063	4.706982
2.497784	289.025473	4.711987
2.944080	277.588036	4.716992
2.814915	284.609689	4.721997
2.766428	283.452977	4.727002
2.965266	277.771270	4.732006
2.719840	291.186163	4.737011
3.059226	278.885944	4.742016
3.040184	285.801757	4.747021
2.887031	280.257458	4.752026
2.791480	277.814134	4.757030
2.867112	286.104013	4.762035
2.924396	273.325975	4.767040
2.757948	280.359795	4.772045
2.901456	290.885328	4.777050
3.115291	300.776582	4.782054
2.934346	307.600710	4.787059
3.463881	299.336152	4.792064
3.048978	287.160439	4.797069
3.163497	276.828526	4.802074
3.052146	289.406156	4.807078
2.976625	285.732143	4.812083
3.341948	287.130208	4.817088
2.771024	290.804192	4.822093
3.278404	301.604916	4.827098
3.064456	299.879336	4.832102
3.338811	309.283381	4.837107
3.702126	301.434011	4.842112
3.346246	289.729944	4.847117
3.429146	280.918436	4.852122
3.245675	279.956882	4.857126
2.825248	279.364652	4.862131
3.267553	269.705892	4.867136
3.048353	289.393617	4.872141
3.289762	293.130151	4.877146
3.162885	300.496304	4.882150
3.028094	294.809917	4.887155
3.308390	299.498986	4.892160
3.357064	298.380834	4.897165
3.497596	300.845514	4.902170
3.326539	305.007348	4.907174
3.160290	299.019001	4.912179
3.648483	303.270534	4.917184
3.440877	308.754230	4.922189
3.379895	307.558345	4.927194
3.405311	304.070997	4.932198
3.505567	299.910691	4.937203
3.304236	307.927597	4.942208
3.455023	311.276533	4.947213
3.760053	311.639996	4.952218
3.439304	309.364831	4.957222
3.171233	309.985769	4.962227
3.346516	298.894505	4.967232
3.272405	316.253128	4.972237
3.221054	302.853003	4.977242
3.368099	299.352926	4.982246
3.322690	305.412328	4.987251
3.515255	305.537145	4.992256
3.229641	298.029901	4.997261
3.255654	310.997315	5.002266
3.536513	322.798499	5.007270
3.576258	330.445445	5.012275
3.879760	332.153760	5.017280
4.249348	331.121367	5.022285
3.658378	322.361638	5.027290
3.728149	313.599628	5.032294
3.394181	304.495916	5.037299
3.521914	321.114229	5.042304
3.392644	326.955821	5.047309
3.545674	320.256210	5.052314
3.750501	325.488627	5.057318
3.277119	332.608524	5.062323
3.840423	325.053680	5.067328
3.676045	328.800017	5.072333
3.539297	327.989329	5.077338
3.937998	333.017364	5.082342
3.873630	326.718812	5.087347
3.856874	324.462454	5.092352
3.625915	329.051299	5.097357
4.078793	325.636178	5.102362
4.334460	330.379735	5.107366
3.794165	332.799231	5.112371
3.901788	322.996726	5.117376
3.642017	329.909144	5.122381
3.840870	326.657211	5.127386
3.921454	326.862850	5.132390
3.547421	333.065500	5.137395
3.917155	332.276697	5.142400
3.592480	332.397134	5.147405
4.123572	330.757300	5.152410
3.803898	334.996211	5.157414
3.695768	342.413228	5.162419
4.308988	350.555631	5.167424
4.191615	350.678390	5.172429
3.961162	336.072423	5.177434
4.021216	330.804754	5.182438
3.494635	344.520007	5.187443
3.900516	351.875474	5.192448
4.105301	364.039787	5.197453
4.188789	358.328671	5.202458
4.380490	356.441450	5.207462
4.077306	359.254074	5.212467
4.309826	353.706273	5.217472
4.352191	353.332598	5.222477
4.262009	353.093587	5.227482
4.331184	351.301495	5.232486
3.906387	347.463894	5.237491
4.498951	342.150752	5.242496
4.082364	347.885506	5.247501
3.998354	357.016691	5.252506
4.319553	352.106738	5.257510
4.592115	353.762954	5.262515
4.226874	352.753945	5.267520
4.191576	342.976985	5.272525
3.949547	352.484107	5.277530
4.103028	353.548369	5.282534
4.205630	354.642748	5.287539
4.235568	356.125005	5.292544
4.027918	362.016855	5.297549
3.976610	360.512562	5.302554
3.997846	353.618449	5.307558
3.820002	358.410955	5.312563
4.574204	360.567518	5.317568
4.258469	365.805579	5.322573
4.385601	361.163315	5.327578
4.308757	373.719778	5.332582
4.612684	382.923073	5.337587
4.501034	368.605353	5.342592
4.239326	385.806772	5.347597
4.448176	384.812216	5.352602
4.761147	380.529977	5.357606
4.345224	381.724585	5.362611
4.426192	385.549553	5.367616
4.254643	385.237868	5.372621
4.517501	391.647638	5.377626
4.816418	381.454455	5.382630
4.268979	388.639762	5.387635
4.465076	384.483403	5.392640
4.316270	388.319062	5.397645
4.375152	385.826215	5.402650
4.869005	385.182481	5.407654
4.530900	393.654296	5.412659
4.654879	383.551797	5.417664
4.359222	378.798599	5.422669
4.753637	382.346661	5.427674
4.917322	387.073007	5.432678
4.729195	391.677304	5.437683
4.993298	383.830788	5.442688
4.817443	382.823742	5.447693
4.784089	389.267267	5.452698
4.639120	379.868145	5.457702
4.672971	389.569346	5.462707
4.966479	378.535441	5.467712
5.033525	381.536837	5.472717
4.650748	389.177242	5.477722
4.567049	379.929874	5.482726
4.402534	394.218031	5.487731
4.699371	390.966553	5.492736
4.647059	386.121441	5.497741
4.908305	378.746781	5.502746
4.842894	382.022035	5.507750
4.661262	383.692470	5.512755
4.896504	376.125730	5.517760
4.844022	382.208413	5.522765
4.949465	376.981076	5.527770
5.075110	387.936578	5.532774
4.592057	382.836248	5.537779
4.941998	382.591553	5.542784
5.283305	389.134566	5.547789
5.117874	383.861082	5.552794
5.046011	390.946565	5.557798
4.481982	386.488518	5.562803
4.775995	395.519364	5.567808
4.826647	403.174124	5.572813
5.018121	410.620158	5.577818
5.226098	401.959839	5.582822
4.873905	413.040845	5.587827
4.992840	410.889768	5.592832
5.296668	415.372698	5.597837
4.850118	412.462322	5.602842
5.057194	411.059912	5.607846
5.230485	412.405815	5.612851
5.217880	406.232005	5.617856
5.219132	414.384900	5.622861
5.410588	412.880531	5.627866
5.208798	403.414368	5.632870
4.777279	408.094770	5.637875
4.755570	407.186958	5.642880
4.856015	409.281442	5.647885
5.473108	413.215407	5.652890
5.120447	414.855693	5.657894
5.077422	408.015921	5.662899
5.067462	404.682794	5.667904
5.104906	412.225730	5.672909
5.241432	412.115716	5.677914
5.445504	406.667270	5.682918
5.268838	408.137608	5.687923
5.239816	415.437856	5.692928
5.434749	413.613398	5.697933
5.287577	406.157184	5.702938
5.548254	405.698681	5.707942
5.143789	411.573928	5.712947
5.496763	409.117258	5.717952
5.490463	416.755636	5.722957
5.403201	412.599375	5.727962
5.298117	403.333198	5.732966
5.247428	423.589464	5.737971
5.798397	426.916849	5.742976
5.436592	415.931812	5.747981
5.931890	408.017423	5.752986
5.603363	407.170340	5.757990
5.411210	413.407797	5.762995
5.406840	413.228108	5.768000
5.576977	409.436485	5.773005
5.347598	416.530839	5.778010
5.548720	403.825085	5.783014
5.492503	415.346945	5.788019
5.449579	409.908723	5.793024
5.576189	429.738577	5.798029
5.376397	435.208433	5.803034
5.622905	432.923467	5.808038
5.733233	444.561623	5.813043
5.678349	441.330443	5.818048
5.513201	438.375972	5.823053
5.641259	442.367583	5.828058
5.850446	433.643783	5.833062
5.357997	439.200623	5.838067
5.943131	433.246366	5.843072
5.713341	434.636444	5.848077
5.382932	435.308283	5.853082
5.940736	429.782260	5.858086
5.794407	430.159497	5.863091
5.556767	433.344684	5.868096
5.738744	433.578731	5.873101
5.302145	435.045505	5.878106
6.018606	433.006452	5.883110
5.776231	426.833834	5.888115
5.948915	438.807071	5.893120
5.939127	430.744016	5.898125
5.909185	429.828002	5.903130
5.973187	430.358948	5.908134
5.349307	434.885996	5.913139
5.666478	434.826773	5.918144
5.714469	437.536930	5.923149
5.743015	433.887711	5.928154
5.954779	435.091544	5.933158
5.670278	442.786178	5.938163
5.956810	450.093947	5.943168
5.912602	453.321598	5.948173
5.965562	455.078672	5.953178
5.920178	455.522352	5.958182
5.742563	462.849064	5.963187
6.043490	461.583809	5.968192
6.060186	462.916286	5.973197
6.171972	462.332412	5.978202
6.275989	469.051841	5.983206
5.921085	471.002537	5.988211
6.095311	468.020198	5.993216
6.352409	465.309618	5.998221
5.927066	459.773108	6.003226
6.360574	459.913960	6.008230
5.907343	453.995837	6.013235
6.241689	444.512088	6.018240
5.792261	438.368743	6.023245
6.008691	451.420322	6.028250
5.973389	455.127478	6.033254
5.769453	465.675914	6.038259
6.024997	460.830003	6.043264
6.065656	466.543774	6.048269
6.267000	464.522150	6.053274
6.430285	473.579846	6.058278
5.781773	459.548654	6.063283
5.963404	460.260492	6.068288
6.028700	470.611720	6.073293
5.869696	464.356422	6.078298
6.267441	470.450851	6.083302
6.025110	468.362699	6.088307
6.239387	459.407130	6.093312
6.221115	457.720479	6.098317
5.893845	452.219227	6.103322
5.833229	451.573778	6.108326
5.961236	470.856119	6.113331
5.989608	465.735746	6.118336
6.035664	458.195450	6.123341
6.074034	466.668425	6.128346
6.341920	462.171764	6.133350
5.975671	469.056626	6.138355
5.983784	459.206361	6.143360
6.264765	467.562229	6.148365
6.101359	469.147556	6.153370
6.251855	464.204206	6.158374
6.233647	460.786938	6.163379
6.313418	443.044394	6.168384
6.027341	438.058720	6.173389
5.782177	446.022444	6.178394
6.084881	436.603770	6.183398
5.869556	441.047823	6.188403
6.258513	446.533005	6.193408
5.789658	450.577014	6.198413
5.910595	455.224654	6.203418
6.421391	458.998110	6.208422
6.350690	456.057312	6.213427
6.415823	436.782618	6.218432
6.078218	430.343340	6.223437
6.152319	442.553492	6.228442
5.892912	432.257931	6.233446
5.960815	438.144597	6.238451
6.062913	436.078414	6.243456
6.126442	441.193797	6.248461
6.108666	445.148146	6.253466
6.458282	441.388508	6.258470
6.151070	439.414930	6.263475
6.072728	442.983292	6.268480
6.272332	444.654111	6.273485
5.901530	448.986483	6.278490
6.202982	445.816531	6.283494
5.972586	451.734121	6.288499
6.320892	440.112614	6.293504
6.310860	443.233667	6.298509
6.064916	443.449339	6.303514
6.301852	443.409015	6.308518
6.174609	438.774948	6.313523
5.996727	433.155381	6.318528
6.041921	439.425263	6.323533
5.636089	445.999936	6.328538
6.212067	434.826824	6.333542
6.009948	439.066324	6.338547
6.060974	438.273667	6.343552
6.154993	430.115252	6.348557
6.206424	441.348175	6.353562
6.410757	445.542976	6.358566
6.052600	450.256187	6.363571
6.191754	444.998238	6.368576
6.164410	435.571165	6.373581
5.943016	437.390206	6.378586
6.004669	434.811495	6.383590
6.259342	438.555473	6.388595
5.685241	442.040157	6.393600
5.998478	437.868595	6.398605
5.974526	441.339848	6.403610
6.345787	442.426942	6.408614
5.946170	450.582549	6.413619
6.057112	439.599358	6.418624
6.224588	447.976164	6.423629
5.771813	441.573910	6.428634
6.271103	437.338396	6.433638
6.022776	447.454007	6.438643
5.854079	446.784363	6.443648
6.053151	443.636781	6.448653
6.274064	446.440070	6.453658
6.211373	441.492163	6.458662
5.770905	447.914074	6.463667
5.805581	446.874037	6.468672
6.284216	442.015324	6.473677
5.884172	452.309736	6.478682
5.845845	437.784316	6.483686
5.829506	447.850924	6.488691
6.132227	442.570511	6.493696
6.334853	443.544818	6.498701
6.147580	433.709362	6.503706
6.095462	438.529647	6.508710
6.182786	441.195676	6.513715
6.560028	431.069288	6.518720
6.173751	427.412297	6.523725
5.722236	420.737766	6.528730
6.118853	432.511395	6.533734
5.965806	436.910887	6.538739
5.979437	435.706466	6.543744
6.401968	439.939846	6.548749
5.926268	437.239680	6.553754
5.754534	432.909984	6.558758
6.081681	436.006681	6.563763
6.339357	442.730499	6.568768
6.343144	434.364753	6.573773
5.805869	419.499901	6.578778
6.305024	417.887209	6.583782
5.959726	413.676463	6.588787
5.900610	410.458606	6.593792
6.365782	426.748897	6.598797
5.946778	419.018887	6.603802
5.871195	408.299062	6.608806
5.525066	410.672326	6.613811
5.899791	427.078030	6.618816
5.745527	432.414199	6.623821
5.594185	439.929778	6.628826
5.984018	433.715050	6.633830
5.854630	439.575680	6.638835
6.053770	435.007538	6.643840
6.283677	439.505219	6.648845
5.677375	437.113424	6.653850
6.120858	437.198928	6.658854
6.268818	438.612079	6.663859
5.533622	441.027324	6.668864
5.849648	444.543387	6.673869
6.003998	438.416175	6.678874
6.074625	439.604157	6.683878
5.835194	438.562775	6.688883
6.153080	449.804575	6.693888
6.008185	449.881026	6.698893
5.618207	455.766671	6.703898
6.315105	463.225288	6.708902
6.179629	461.898693	6.713907
6.284273	458.699463	6.718912
6.268246	454.342201	6.723917
5.909949	447.355655	6.728922
6.249947	435.982230	6.733926
6.418155	442.682100	6.738931
5.831930	435.756582	6.743936
6.117113	442.232476	6.748941
6.039786	438.637811	6.753946
6.401993	442.001102	6.758950
6.104323	439.342647	6.763955
5.910480	441.897703	6.768960
6.093338	438.338202	6.773965
6.347068	440.652286	6.778970
6.170565	445.324379	6.783974
6.082341	441.595377	6.788979
6.181506	445.395359	6.793984
6.232679	436.712134	6.798989
6.303911	443.749908	6.803994
6.548286	440.386416	6.808998
6.114532	448.354379	6.814003
6.141202	440.114761	6.819008
6.291191	448.272841	6.824013
5.947390	435.934023	6.829018
5.869719	430.352540	6.834022
6.047283	437.702687	6.839027
5.993908	434.661100	6.844032
6.124254	436.643332	6.849037
6.159948	444.585196	6.854042
6.178304	443.452803	6.859046
6.062247	446.289906	6.864051
6.080450	435.729379	6.869056
5.630232	437.476703	6.874061
5.437100	436.472360	6.879066
5.767012	435.215221	6.884070
5.508638	449.166945	6.889075
6.045134	444.647185	6.894080
5.932541	438.738971	6.899085
5.611111	442.737732	6.904090
6.098743	445.344205	6.909094
5.835983	454.161754	6.914099
5.942880	454.157624	6.919104
5.889858	455.864863	6.924109
6.148102	464.018644	6.929114
6.062528	463.440381	6.934118
5.805079	468.267535	6.939123
6.060978	471.913250	6.944128
6.323592	461.058144	6.949133
6.089872	465.065315	6.954138
6.236326	466.602093	6.959142
6.007060	465.875498	6.964147
6.146566	464.619715	6.969152
6.366487	452.186233	6.974157
6.075879	447.169628	6.979162
5.994202	437.406212	6.984166
5.969348	440.969356	6.989171
5.814502	449.608641	6.994176
6.175678	450.004440	6.999181
6.131501	452.956835	7.004186
6.303593	438.945785	7.009190
6.098885	443.226821	7.014195
6.236139	434.175763	7.019200
6.299460	434.678342	7.024205
5.937337	436.519432	7.029210
6.285009	436.540853	7.034214
6.149436	437.334028	7.039219
6.320499	435.329807	7.044224
6.079647	439.695600	7.049229
6.040786	440.144586	7.054234
6.002665	435.370004	7.059238
5.710670	438.155577	7.064243
5.989770	435.938273	7.069248
5.941577	430.769794	7.074253
5.766569	437.267169	7.079258
5.749357	432.925918	7.084262
5.862559	444.380123	7.089267
6.106966	445.123253	7.094272
6.380869	451.695833	7.099277
6.134561	446.650141	7.104282
6.399635	441.786923	7.109286
6.164018	437.821582	7.114291
5.974396	433.861691	7.119296
6.123901	435.179685	7.124301
6.101034	440.438321	7.129306
6.132269	436.010382	7.134310
5.951635	446.805097	7.139315
5.920812	442.839306	7.144320
5.780964	439.453756	7.149325
5.769613	449.063994	7.154330
5.900898	432.588406	7.159334
5.815813	444.937399	7.164339
6.150229	454.569396	7.169344
6.069783	467.588406	7.174349
6.034913	466.900957	7.179354
6.381811	469.111860	7.184358
5.936623	456.627558	7.189363
6.263949	456.263017	7.194368
6.092732	446.086510	7.199373
5.774218	447.462016	7.204378
6.335286	447.605029	7.209382
6.339531	444.636671	7.214387
6.545488	433.388655	7.219392
6.400924	439.112455	7.224397
6.356458	447.240890	7.229402
6.384092	436.216968	7.234406
5.995984	439.324491	7.239411
6.056347	450.344044	7.244416
6.293664	438.309650	7.249421
6.364744	442.550639	7.254426
5.962154	439.535292	7.259430
5.877183	437.216840	7.264435
5.920792	439.918192	7.269440
6.668541	443.445708	7.274445
6.034763	441.770074	7.279450
6.145115	433.786272	7.284454
6.145000	432.476436	7.289459
5.638608	432.543086	7.294464
6.101138	438.393232	7.299469
5.959410	441.443169	7.304474
6.120943	441.702566	7.309478
6.129504	449.677158	7.314483
5.851272	440.767127	7.319488
6.261799	435.311635	7.324493
5.964576	448.766400	7.329498
6.161337	440.614030	7.334502
5.960847	447.264100	7.339507
6.078218	439.469025	7.344512
6.241793	449.124623	7.349517
6.299306	440.918138	7.354522
5.957346	434.311859	7.359526
5.815576	429.635777	7.364531
5.819961	434.194103	7.369536
5.824555	434.272442	7.374541
5.741305	442.524012	7.379546
6.186328	439.315748	7.384550
6.097466	442.638980	7.389555
5.808079	447.376218	7.394560
6.362647	439.446202	7.399565
5.984582	443.969539	7.404570
6.106895	445.329760	7.409574
6.149684	441.434694	7.414579
5.842990	440.457636	7.419584
6.040924	437.019163	7.424589
5.836632	440.575620	7.429594
5.963489	441.406772	7.434598
6.128478	442.456580	7.439603
6.372221	450.517713	7.444608
6.263925	441.470322	7.449613
6.012128	438.630669	7.454618
6.163166	431.428283	7.459622
6.332385	445.733795	7.464627
6.152058	448.533512	7.469632
6.428201	431.908675	7.474637
5.841778	435.433254	7.479642
6.478347	436.791995	7.484646
6.136790	421.675009	7.489651
5.963281	419.183767	7.494656
6.014891	412.088717	7.499661
5.852614	409.810855	7.504666
6.007625	421.188890	7.509670
6.282852	432.494312	7.514675
6.113444	428.540747	7.519680
6.229702	417.196062	7.524685
5.914833	415.239505	7.529690
6.165160	408.527780	7.534694
6.025952	413.595825	7.539699
5.926899	414.943271	7.544704
6.163723	410.100306	7.549709
5.971850	413.316285	7.554714
6.449792	404.496605	7.559718
6.109429	423.469460	7.564723
6.003422	413.051796	7.569728
5.995967	416.795711	7.574733
5.747843	421.694158	7.579738
5.988732	423.374326	7.584742
6.044278	417.392318	7.589747
5.856157	417.276221	7.594752
6.447081	427.130610	7.599757
5.934758	419.374092	7.604762
6.229847	408.393705	7.609766
6.238109	411.831431	7.614771
6.069061	415.499422	7.619776
5.957699	408.306519	7.624781
5.772184	412.283979	7.629786
6.075408	405.997408	7.634790
6.014241	417.469424	7.639795
5.977846	415.019976	7.644800
6.256491	414.248605	7.649805
6.054152	414.969981	7.654810
5.989477	411.101251	7.659814
5.879693	409.523857	7.664819
5.867379	422.449900	7.669824
5.751165	429.773306	7.674829
6.476152	435.288095	7.679834
6.200381	427.124345	7.684838
6.021966	425.567194	7.689843
6.062732	435.131293	7.694848
6.315585	427.432056	7.699853
6.046998	427.686077	7.704858
6.375029	412.328143	7.709862
6.056088	415.200194	7.714867
5.824020	416.011651	7.719872
6.140723	409.830536	7.724877
5.875138	420.983401	7.729882
5.944269	417.353137	7.734886
5.856585	422.599776	7.739891
6.201677	418.688988	7.744896
6.393460	428.514165	7.749901
6.256213	418.427265	7.754906
6.381213	404.895028	7.759910
6.023878	413.847600	7.764915
5.981213	415.594342	7.769920
6.180953	411.965762	7.774925
5.751661	418.819352	7.779930
5.673115	409.533195	7.784934
6.070387	406.411513	7.789939
5.972145	416.728222	7.794944
5.897085	407.530106	7.799949
6.140445	416.249354	7.804954
5.986979	424.483443	7.809958
6.177118	422.406632	7.814963
6.352770	412.827540	7.819968
5.899169	414.600702	7.824973
5.690073	416.107760	7.829978
5.926730	426.894030	7.834982
6.336059	435.922648	7.839987
5.853593	428.677149	7.844992
6.155953	436.634176	7.849997
5.905106	435.746446	7.855002
6.267164	437.268423	7.860006
6.228920	437.337655	7.865011
5.943526	419.753590	7.870016
6.201429	413.186211	7.875021
5.865123	421.907699	7.880026
6.156112	424.367805	7.885030
5.992757	410.232163	7.890035
6.030733	422.166383	7.895040
5.871123	427.604630	7.900045
6.111531	437.308296	7.905050
6.333163	444.021943	7.910054
6.001440	425.818697	7.915059
5.780686	423.151356	7.920064
6.179577	426.524716	7.925069
6.208422	437.574510	7.930074
6.020361	431.026378	7.935078
6.203868	427.881237	7.940083
6.025518	422.128867	7.945088
6.034026	423.684091	7.950093
6.030561	422.121676	7.955098
6.381963	415.539646	7.960102
6.241127	414.878294	7.965107
5.816751	420.136556	7.970112
6.253944	418.362727	7.975117
6.088919	418.907411	7.980122
6.117310	415.069619	7.985139
5.910850	410.870089	7.990157
6.168303	424.920076	7.995174
6.115078	412.573671	8.000192
5.711006	422.905710	8.005210
6.096606	416.994521	8.010227
5.854988	412.797344	8.015245
6.139760	423.851413	8.020262
6.024786	419.984679	8.025280
6.124234	436.997423	8.030298
6.054578	435.534569	8.035315
5.965153	437.757561	8.040333
5.982700	446.685521	8.045350
6.115425	442.918824	8.050368
6.093176	444.799939	8.055386
5.778804	447.086579	8.060403
6.053186	444.351704	8.065421
6.098955	444.742120	8.070438
6.104329	439.070375	8.075456
6.158810	441.457009	8.080474
6.328494	434.509848	8.085491
6.277855	440.892340	8.090509
6.094464	452.650927	8.095526
6.458360	447.257515	8.100544
6.122056	442.939470	8.105562
6.284338	437.779617	8.110579
6.205082	437.697326	8.115597
5.995480	444.584398	8.120614
6.198441	444.063421	8.125632
6.007575	443.032960	8.130650
6.171875	443.013492	8.135667
6.012128	438.320653	8.140685
6.212484	443.543532	8.145702
6.280468	436.208370	8.150720
6.277961	439.471761	8.155738
6.194166	445.266170	8.160755
5.971008	446.828477	8.165773
6.284339	449.417546	8.170790
6.243100	435.185270	8.175808
6.220626	444.024826	8.180826
6.496643	443.249411	8.185843
6.143138	439.082381	8.190861
6.150775	446.064802	8.195878
6.401527	439.587766	8.200896
6.255628	444.543011	8.205914
6.143576	447.956108	8.210931
6.332984	443.066553	8.215949
5.872570	450.529401	8.220966
6.080477	441.824812	8.225984
6.085765	442.515054	8.231002
5.870344	448.450005	8.236019
6.365664	463.592509	8.241037
6.331530	471.853249	8.246054
6.458263	469.933597	8.251072
6.485350	478.986307	8.256090
6.378774	463.871169	8.261107
6.239924	453.873402	8.266125
6.390060	460.309647	8.271142
6.526562	466.593400	8.276160
6.852896	466.652684	8.281178
6.602639	451.137198	8.286195
6.668581	454.074293	8.291213
6.387931	455.920158	8.296230
6.503232	445.282984	8.301248
6.551569	442.671887	8.306266
6.390287	449.690243	8.311283
6.490026	436.994812	8.316301
6.235900	436.794756	8.321318
6.472653	440.819062	8.326336
6.357043	444.516732	8.331354
6.307141	446.651484	8.336371
6.239202	444.206925	8.341389
6.017227	446.816752	8.346406
6.050521	446.016252	8.351424
6.406427	445.613320	8.356442
6.518186	444.406058	8.361459
6.581638	443.679726	8.366477
6.256285	453.096907	8.371494
6.239880	452.787022	8.376512
6.700999	461.752785	8.381530
6.475945	473.293856	8.386547
6.633124	455.082637	8.391565
6.058366	461.622994	8.396582
6.524113	456.529195	8.401600
6.844859	456.986978	8.406618
6.654788	464.394851	8.411635
6.442610	448.475777	8.416653
6.317061	449.328527	8.421670
6.661763	455.008466	8.426688
6.370191	454.583907	8.431706
6.131834	463.072297	8.436723
6.722526	467.681769	8.441741
6.672407	469.289548	8.446758
6.744075	465.147412	8.451776
6.482703	471.543998	8.456794
6.391818	477.967522	8.461811
6.723041	467.179741	8.466829
6.533440	479.194934	8.471846
6.527247	475.853932	8.476864
6.574599	474.786145	8.481882
6.455662	474.681669	8.486899
6.665538	469.937220	8.491917
6.040749	481.045475	8.496934
6.852755	467.787152	8.501952
6.604574	477.782379	8.506970
6.755624	474.495634	8.511987
6.729184	472.274939	8.517005
6.413398	480.055958	8.522022
6.474987	469.398784	8.527040
6.813909	471.595691	8.532058
6.734545	477.064374	8.537075
6.592885	472.365536	8.542093
6.502260	477.201679	8.547110
6.536194	465.412771	8.552128
6.754936	474.624795	8.557146
6.441512	465.730484	8.562163
6.724675	463.786322	8.567181
6.539799	464.216032	8.572199
6.933331	460.796624	8.577216
6.764606	474.376948	8.582234
6.745292	475.298259	8.587251
6.611680	470.187914	8.592269
6.711437	474.208446	8.597287
6.699079	465.058684	8.602304
6.624362	467.847409	8.607322
6.762250	476.052797	8.612339
6.624627	469.150617	8.617357
6.850662	474.978540	8.622375
6.584404	469.699633	8.627392
6.801003	466.339504	8.632410
6.758649	476.955721	8.637427
6.753532	461.859400	8.642445
6.691380	473.980851	8.647463
6.521453	479.296469	8.652480
6.607089	475.388824	8.657498
6.526694	475.448719	8.662515
6.675071	468.119883	8.667533
6.827150	463.842074	8.672551
6.819752	478.381717	8.677568
6.990411	470.661232	8.682586
7.025552	473.849303	8.687603
6.939239	466.219575	8.692621
6.502088	472.287103	8.697639
6.696023	464.534572	8.702656
6.896890	477.167070	8.707674
6.662211	475.095764	8.712691
6.686190	467.745395	8.717709
6.535088	475.529011	8.722727
6.896723	468.684304	8.727744
7.194608	479.013687	8.732762
6.877489	482.203305	8.737779
6.999941	471.561839	8.742797
6.820756	478.642970	8.747815
6.538491	467.181310	8.752832
6.797788	469.542168	8.757850
6.755248	490.667056	8.762867
6.891832	481.209932	8.767885
6.687651	484.615381	8.772903
6.994209	496.698011	8.777920
7.040583	497.479646	8.782938
6.801792	500.429781	8.787955
6.551395	496.079328	8.792973
6.812773	499.080481	8.797991
6.590505	496.085749	8.803008
6.664402	485.354055	8.808026
6.887103	492.302797	8.813043
6.926652	492.650007	8.818061
7.078739	495.718776	8.823079
6.907775	493.186213	8.828096
7.253227	492.993197	8.833114
6.798331	500.619300	8.838131
6.974217	487.779361	8.843149
6.636086	492.341868	8.848167
7.162511	498.201628	8.853184
6.861860	489.794444	8.858202
6.555286	496.860828	8.863219
7.169075	493.050305	8.868237
7.217821	487.807243	8.873255
6.951841	495.735097	8.878272
7.099826	499.006477	8.883290
7.300774	501.556360	8.888307
7.267397	495.392060	8.893325
6.922631	495.938339	8.898343
6.722035	497.187851	8.903360
7.174423	486.914396	8.908378
6.972425	499.714171	8.913395
7.181467	490.662248	8.918413
7.069018	489.426998	8.923431
6.833768	496.497985	8.928448
7.198710	504.273342	8.933466
7.091840	503.722015	8.938483
7.297597	498.466972	8.943501
6.957178	499.173513	8.948519
6.989034	496.555523	8.953536
7.409015	504.685168	8.958554
7.173402	503.945733	8.963571
6.769227	499.329044	8.968589
7.231252	510.112401	8.973607
7.238199	516.340733	8.978624
7.321833	516.756774	8.983642
7.139562	523.393445	8.988659
7.402073	509.514298	8.993677
7.230752	500.118030	8.998695
6.988593	494.974193	9.003712
7.042016	493.820249	9.008730
7.162379	512.751640	9.013747
7.262892	505.657502	9.018765
7.462486	506.219474	9.023783
7.288104	499.531321	9.028800
7.225189	491.626521	9.033818
7.047837	502.295461	9.038835
7.100856	497.149555	9.043853
7.453011	510.440015	9.048871
7.229436	508.351186	9.053888
7.452663	497.390963	9.058906
6.939984	502.362667	9.063923
7.078063	502.612391	9.068941
7.367882	515.205732	9.073959
7.189148	521.702995	9.078976
7.189032	520.611086	9.083994
7.367553	521.280500	9.089011
7.486986	511.876539	9.094029
7.361369	520.757540	9.099047
7.322655	524.414777	9.104064
7.297106	511.237159	9.109082
7.174115	517.214455	9.114099
7.190164	523.163656	9.119117
7.763077	514.897295	9.124135
7.711589	513.267490	9.129152
7.477474	496.726971	9.134170
7.226309	496.898829	9.139187
7.073534	502.265415	9.144205
7.080525	498.376398	9.149223
6.922193	514.965710	9.154240
7.382535	521.754155	9.159258
7.679711	520.808166	9.164275
7.253026	518.422962	9.169293
7.357290	525.592242	9.174311
7.366335	525.063777	9.179328
7.892204	521.582598	9.184346
7.611806	523.453677	9.189363
7.231454	511.628665	9.194381
7.787773	509.130469	9.199399
6.906487	514.036855	9.204416
7.520738	520.296265	9.209434
7.343580	522.681334	9.214451
7.392126	526.694122	9.219469
7.511032	522.932730	9.224487
7.425522	528.954649	9.229504
7.303698	516.912405	9.234522
7.327408	529.200318	9.239539
7.253657	524.828492	9.244557
7.410990	526.687790	9.249575
7.224666	532.362594	9.254592
7.500653	525.673293	9.259610
7.432549	526.971475	9.264627
7.142718	526.691807	9.269645
7.150697	521.679181	9.274663
7.133685	520.984388	9.279680
7.363422	530.933165	9.284698
7.903147	550.313278	9.289715
7.769650	542.839230	9.294733
7.750732	531.443562	9.299751
7.481168	528.399431	9.304768
7.577385	526.162667	9.309786
7.458256	529.109837	9.314803
7.451453	528.801602	9.319821
7.626832	536.076507	9.324839
7.235454	546.728515	9.329856
7.765378	555.942318	9.334874
7.916913	552.967902	9.339891
7.562231	543.682390	9.344909
7.927616	541.289843	9.349927
7.241266	543.527481	9.354944
7.148452	538.338142	9.359962
7.425328	538.727062	9.364979
7.591750	553.138547	9.369997
8.058850	545.453632	9.375015
7.273487	554.621054	9.380032
7.774339	549.960380	9.385050
7.378172	547.889121	9.390067
7.382366	550.340453	9.395085
7.644209	551.454398	9.400103
7.074945	562.364658	9.405120
7.427230	553.094602	9.410138
7.701357	559.729205	9.415155
7.732257	557.101889	9.420173
7.462713	554.979233	9.425191
7.386570	580.038414	9.430208
7.913764	583.616463	9.435226
7.689189	581.284789	9.440243
7.670117	587.589804	9.445261
8.168537	578.296839	9.450279
7.663579	589.162326	9.455296
7.782488	588.168527	9.460314
8.044630	581.216291	9.465331
7.628664	576.598273	9.470349
8.006199	575.087432	9.475367
7.777653	562.774704	9.480384
8.019834	564.267266	9.485402
7.590709	565.801895	9.490419
7.428119	564.230517	9.495437
7.764778	563.808508	9.500455
7.871611	583.019800	9.505472
8.020565	588.941888	9.510490
8.104762	578.950129	9.515507
7.859637	573.866693	9.520525
8.070899	579.050034	9.525543
7.460089	572.218797	9.530560
7.615636	567.728984	9.535578
7.969290	577.917145	9.540595
8.025891	577.983978	9.545613
8.413533	584.215800	9.550631
7.678737	571.628940	9.555648
7.589492	580.639970	9.560666
7.816234	577.802088	9.565683
7.771966	590.753937	9.570701
7.816450	593.820648	9.575719
7.645918	593.197242	9.580736
7.771911	585.717233	9.585754
7.702494	592.096409	9.590771
7.688439	593.809000	9.595789
8.082968	581.676342	9.600807
7.936202	589.749659	9.605824
7.896297	591.945977	9.610842
7.990170	583.729395	9.615859
8.133982	594.174503	9.620877
8.374217	585.051374	9.625895
7.993196	587.042365	9.630912
8.066545	583.808799	9.635930
8.059461	581.607147	9.640947
8.258094	581.105780	9.645965
8.160847	572.830787	9.650983
8.048325	587.743590	9.656000
8.098768	587.429540	9.661018
8.429531	589.413149	9.666035
8.118637	587.937588	9.671053
7.765527	577.105486	9.676071
7.516780	582.682791	9.681088
7.549627	588.219132	9.686106
7.972545	577.991267	9.691123
7.527329	584.287312	9.696141
8.259870	591.478098	9.701159
7.908499	585.704414	9.706176
7.935735	598.941708	9.711194
8.495975	599.169469	9.716211
8.335712	600.945994	9.721229
8.063420	587.778578	9.726247
8.339010	585.406406	9.731264
8.090290	592.634175	9.736282
8.141899	573.663058	9.741299
7.710328	594.707014	9.746317
7.785953	591.507803	9.751335
8.491387	605.222658	9.756352
8.223351	604.027556	9.761370
8.652678	604.032834	9.766387
8.141331	595.664924	9.771405
8.589781	585.805435	9.776423
8.155819	581.111342	9.781440
8.173332	584.131784	9.786458
8.127099	576.151750	9.791475
7.990693	581.963914	9.796493
8.345546	589.008751	9.801511
8.345922	603.256946	9.806528
8.239876	586.226069	9.811546
8.057205	588.324836	9.816563
8.309420	601.015648	9.821581
8.422995	600.767445	9.826599
8.333109	592.494445	9.831616
8.211906	602.362550	9.836634
8.439515	597.044095	9.841651
7.992973	594.359038	9.846669
8.608016	598.507143	9.851687
8.163701	607.371850	9.856704
8.370590	607.216322	9.861722
8.311953	605.051147	9.866739
8.291107	602.526606	9.871757
8.557781	600.383044	9.876775
8.584023	603.339007	9.881792
7.863093	592.147965	9.886810
8.403222	580.740412	9.891827
7.936425	598.826629	9.896845
8.206291	598.727505	9.901863
8.165279	611.994437	9.906880
8.323451	605.989433	9.911898
8.256722	609.660545	9.916915
8.213661	610.165866	9.921933
8.197738	599.290388	9.926951
8.175951	606.757158	9.931968
8.110418	614.543207	9.936986
8.774891	618.421643	9.942003
8.306096	605.184018	9.947021
8.403319	595.707754	9.952039
8.383080	593.356686	9.957056
8.494977	616.843286	9.962074
8.867957	619.965828	9.967091
8.441997	606.948706	9.972109
8.642936	604.184289	9.977127
8.515171	607.757667	9.982144
8.462786	613.468315	9.987162
9.034289	606.751617	9.992179
8.364205	602.801406	9.997197
8.169495	604.545459	10.002215
8.267159	610.832192	10.007232
8.833140	617.291701	10.012250
8.456165	604.361579	10.017267
8.720268	611.840362	10.022285
8.747334	615.922807	10.027303
8.556181	609.164658	10.032320
8.540723	605.572621	10.037338
8.629572	605.697517	10.042355
8.618002	610.761148	10.047373
8.693315	602.105658	10.052391
8.701640	609.100658	10.057408
8.452208	617.644504	10.062426
8.704426	601.627286	10.067443
8.497761	610.634638	10.072461
8.437213	607.384177	10.077479
8.522753	614.445975	10.082496
8.718957	626.912054	10.087514
8.899406	624.475889	10.092531
8.582712	635.665353	10.097549
8.568993	634.357820	10.102567
9.037648	631.677684	10.107584
8.749563	628.434468	10.112602
8.692235	606.365637	10.117619
8.433936	607.889282	10.122637
8.697798	625.453951	10.127655
8.903061	631.648095	10.132672
8.686484	635.191212	10.137690
8.980368	629.843429	10.142707
8.797109	622.983053	10.147725
8.406750	621.668261	10.152743
8.508114	628.771766	10.157760
8.852741	642.719904	10.162778
8.703874	640.695094	10.167795
8.788361	632.577790	10.172813
8.595410	633.150778	10.177831
8.845170	636.560870	10.182848
8.341577	632.527762	10.187866
8.861812	638.505302	10.192883
8.832724	627.284734	10.197901
8.732548	632.655740	10.202919
8.642388	629.198479	10.207936
8.500914	641.089476	10.212954
8.467694	636.105364	10.217971
8.895053	639.301439	10.222989
8.703734	643.651635	10.228007
8.876331	649.450119	10.233024
8.830888	663.790748	10.238042
8.993100	664.323868	10.243059
9.159101	659.949158	10.248077
8.958503	652.981035	10.253095
9.055842	644.659742	10.258112
8.882222	637.406534	10.263130
8.849538	637.537849	10.268147
9.078814	640.411514	10.273165
8.618127	643.604720	10.278183
8.929868	653.225139	10.283200
8.746328	656.422261	10.288218
9.081213	659.658075	10.293235
8.821829	659.616629	10.298253
9.119293	658.206688	10.303271
9.100852	656.420215	10.308288
8.777727	673.748700	10.313306
9.132082	660.558785	10.318323
8.903661	664.744387	10.323341
8.954506	664.054736	10.328359
9.289301	663.203831	10.333376
9.113675	666.683734	10.338394
8.873110	670.189592	10.343411
8.975197	668.911248	10.348429
9.049080	669.092137	10.353447
9.338883	658.462209	10.358464
9.118941	664.681960	10.363482
8.796226	661.557773	10.368499
9.018887	663.043935	10.373517
9.045191	669.395517	10.378535
9.247820	657.810423	10.383552
9.126646	670.073797	10.388570
9.280641	661.434353	10.393587
9.471482	661.795732	10.398605
9.177120	667.156149	10.403623
9.116485	659.172023	10.408640
9.185933	673.876507	10.413658
9.336193	667.266813	10.418675
9.219461	666.483498	10.423693
9.371801	673.746290	10.428711
9.057307	669.437395	10.433728
8.757261	672.510763	10.438746
9.156676	666.616263	10.443763
9.352144	662.524111	10.448781
9.016785	678.071502	10.453799
9.692003	669.536580	10.458816
9.319851	670.001948	10.463834
9.274568	661.188601	10.468851
9.186509	662.597216	10.473869
9.332285	669.330863	10.478887
9.643320	667.347600	10.483904
9.208369	661.426042	10.488922
9.115646	660.105638	10.493939
9.434661	659.768442	10.498957
9.155871	666.101555	10.503975
9.167755	662.669323	10.508992
9.426559	668.905583	10.514010
9.415516	660.645445	10.519027
9.393324	660.065066	10.524045
9.032110	661.491233	10.529063
9.354440	664.337698	10.534080
9.201667	661.483527	10.539098
9.112031	669.459567	10.544115
9.075720	660.840473	10.549133
9.073275	663.232900	10.554151
9.541398	664.181990	10.559168
9.566661	676.883168	10.564186
9.410206	671.788967	10.569203
9.406317	675.787915	10.574221
9.471182	682.054566	10.579239
9.903373	683.167076	10.584256
9.476586	677.455671	10.589274
9.303817	660.495137	10.594291
9.730879	661.195042	10.599309
9.284101	659.614534	10.604327
9.237090	653.190387	10.609344
9.374928	673.024918	10.614362
9.414924	680.800772	10.619379
9.676883	682.542709	10.624397
9.683046	686.391762	10.629415
9.749488	684.169111	10.634432
9.748626	689.477237	10.639450
9.398630	675.826473	10.644467
9.717497	680.052560	10.649485
9.557508	681.598678	10.654503
9.409826	673.363098	10.659520
9.679212	672.948472	10.664538
9.626579	678.514013	10.669555
9.610488	681.416661	10.674573
9.556425	688.134290	10.679591
9.892669	686.737207	10.684608
9.853257	678.238510	10.689626
9.423812	672.293995	10.694643
9.539393	673.796935	10.699661
9.683115	690.613637	10.704679
9.672008	692.723405	10.709696
9.446728	689.132669	10.714714
9.348809	696.816531	10.719731
9.881691	686.577687	10.724749
9.779244	691.368403	10.729767
9.640625	684.851301	10.734784
9.875871	686.562709	10.739802
9.875451	693.761082	10.744819
9.924217	683.784283	10.749837
9.669517	690.056825	10.754855
9.487968	689.697072	10.759872
9.761463	688.852615	10.764890
9.638273	691.169291	10.769907
9.728141	684.774178	10.774925
10.192242	705.400220	10.779943
9.883215	694.848317	10.784960
10.029781	696.908134	10.789978
9.862600	698.433289	10.794995
9.811991	691.201811	10.800013
9.986357	694.850943	10.805031
9.904632	690.101632	10.810048
9.725841	697.454185	10.815066
9.916685	690.554103	10.820083
10.084898	686.450437	10.825101
9.906544	693.891283	10.830119
9.805509	692.976119	10.835136
9.696378	694.810914	10.840154
9.555313	699.800185	10.845171
9.566977	695.313950	10.850189
9.354381	698.256857	10.855207
9.561746	698.539908	10.860224
9.632605	695.379295	10.865242
9.632437	695.139445	10.870259
10.143086	705.785916	10.875277
9.725592	717.764393	10.880295
9.905557	720.137714	10.885312
9.925197	718.266373	10.890330
9.774451	723.093067	10.895347
9.879913	727.014932	10.900365
9.831536	725.990532	10.905383
9.890021	728.051530	10.910400
9.864986	731.984376	10.915418
9.781817	721.371823	10.920435
9.783110	721.090718	10.925453
9.805379	730.390463	10.930471
9.885025	731.529811	10.935488
9.954537	721.354081	10.940506
10.004033	739.047122	10.945523
10.098332	735.633522	10.950541
10.044035	736.951646	10.955559
10.162250	744.071492	10.960576
9.938403	740.600441	10.965594
10.086924	741.949904	10.970611
10.167989	745.799857	10.975629
10.171247	759.833131	10.980647
10.130157	746.048707	10.985664
10.387711	744.010699	10.990682
10.065262	748.779096	10.995699
10.397254	740.629275	11.000717
10.306392	757.246110	11.005735
10.189515	746.402139	11.010752
10.264398	745.970648	11.015770
9.977378	750.730339	11.020787
10.443822	744.796909	11.025805
10.195823	747.909473	11.030823
10.562161	739.782673	11.035840
10.463975	745.652017	11.040858
10.312198	736.429287	11.045875
10.321512	725.546621	11.050893
10.153439	725.866407	11.055911
10.132332	738.909408	11.060928
10.110352	736.943601	11.065946
10.066459	749.144428	11.070963
10.329465	747.086630	11.075981
10.302836	743.856076	11.080999
10.522161	752.124571	11.086016
10.445307	742.113773	11.091034
10.358770	746.772623	11.096051
10.342271	740.675022	11.101069
10.183411	750.097830	11.106087
10.004204	741.532644	11.111104
9.891947	752.604943	11.116122
9.788930	751.920461	11.121139
10.338482	748.034743	11.126157
10.093673	745.513714	11.131175
10.210525	761.227008	11.136192
10.621184	764.327893	11.141210
10.693668	766.667569	11.146227
10.278811	768.461910	11.151245
10.530580	773.834620	11.156263
10.526895	770.916046	11.161280
10.871331	764.660900	11.166298
10.364123	767.526902	11.171315
10.384890	773.857299	11.176333
10.242002	779.291846	11.181351
10.338543	779.077868	11.186368
10.440854	770.525364	11.191386
10.388425	772.587967	11.196403
10.433858	774.505849	11.201421
10.340905	778.553488	11.206439
10.403054	774.674703	11.211456
10.365672	770.439130	11.216474
10.570267	774.556912	11.221491
10.875822	771.267995	11.226509
10.635327	775.269323	11.231527
10.673406	768.528845	11.236544
11.070771	766.421592	11.241562
10.833158	769.459948	11.246579
10.655123	766.231022	11.251597
10.668822	763.757850	11.256615
10.799959	764.986962	11.261632
11.312099	768.924013	11.266650
10.780899	776.663173	11.271667
11.034564	765.335101	11.276685
10.949999	771.278058	11.281703
10.713835	767.897294	11.286720
10.772775	754.965034	11.291738
10.576386	761.449371	11.296755
10.715757	776.512213	11.301773
10.569900	774.228140	11.306791
10.650611	777.825692	11.311808
11.046908	771.666558	11.316826
10.602302	780.780704	11.321843
10.807182	782.623112	11.326861
10.700429	774.257997	11.331879
10.875721	782.779557	11.336896
11.138534	776.306822	11.341914
10.954589	773.801499	11.346931
10.926214	761.258455	11.351949
10.965103	764.528043	11.356967
10.715072	782.268057	11.361984
10.888048	769.065456	11.367002
10.851485	777.168928	11.372019
10.721792	778.833383	11.377037
10.812159	782.003390	11.382055
10.915931	776.183578	11.387072
11.023238	776.845225	11.392090
10.932571	784.963489	11.397107
10.900772	788.446127	11.402125
10.983222	779.069911	11.407143
10.748138	779.930371	11.412160
10.913572	765.596022	11.417178
10.688221	770.784712	11.422195
10.758163	773.086917	11.427213
10.771781	782.618417	11.432231
10.921370	785.141674	11.437248
11.356550	776.442339	11.442266
10.767170	784.667144	11.447283
10.755760	774.794396	11.452301
10.785459	774.250064	11.457319
11.265239	788.170830	11.462336
11.073203	789.469514	11.467354
10.996131	791.842092	11.472371
11.050357	800.502550	11.477389
11.254067	798.709657	11.482407
11.139993	809.040662	11.487424
11.297045	799.305608	11.492442
11.139862	790.329849	11.497459
10.949945	782.268095	11.502477
11.463379	795.460914	11.507495
11.398953	791.535686	11.512512
11.445322	775.257076	11.517530
11.149694	777.809063	11.522547
10.856128	778.798606	11.527565
10.848836	778.828114	11.532583
10.879455	795.757310	11.537600
11.376424	790.664838	11.542618
11.192406	809.429639	11.547635
11.203976	806.199401	11.552653
11.145759	793.910319	11.557671
11.248493	809.584843	11.562688
11.358781	805.458668	11.567706
10.855182	795.981761	11.572723
11.180416	793.242023	11.577741
11.267200	800.912769	11.582759
11.365547	802.743468	11.587776
11.242876	800.070751	11.592794
11.210483	795.458849	11.597811
11.056332	802.719222	11.602829
11.061362	796.349986	11.607847
11.025868	804.020957	11.612864
11.550934	813.904686	11.617882
11.716072	825.877154	11.622899
11.431788	809.047560	11.627917
11.436240	803.940733	11.632935
11.091360	804.698477	11.637952
11.347543	815.009343	11.642970
11.633924	817.848843	11.647987
11.598862	827.536317	11.653005
11.554275	808.687321	11.658023
11.123490	821.526328	11.663040
11.729298	822.292908	11.668058
11.833026	826.271871	11.673075
11.779452	815.045555	11.678093
11.293354	808.122103	11.683111
11.310123	804.843713	11.688128
11.610818	817.893157	11.693146
11.575701	818.728599	11.698163
11.810694	814.762764	11.703181
11.483280	811.317394	11.708199
11.593557	820.123714	11.713216
11.770576	825.085273	11.718234
11.728103	805.529047	11.723251
11.361525	806.788808	11.728269
11.671319	807.828985	11.733287
11.508319	818.167661	11.738304
11.778485	815.771062	11.743322
11.339980	816.306790	11.748339
11.546423	816.732000	11.753357
11.675298	825.260853	11.758375
11.743091	833.354311	11.763392
11.753009	832.787830	11.768410
11.960846	825.623101	11.773427
11.632053	831.231959	11.778445
11.796135	821.521038	11.783463
11.289255	823.405542	11.788480
11.855028	815.575664	11.793498
11.685736	827.082980	11.798515
11.445412	832.873637	11.803533
11.949023	828.584844	11.808551
11.751726	827.066218	11.813568
11.449216	822.894263	11.818586
11.773204	829.903007	11.823603
11.654923	829.441819	11.828621
11.774032	821.117034	11.833639
11.726729	826.265219	11.838656
11.542757	824.132279	11.843674
11.988457	824.804024	11.848691
11.432424	829.817324	11.853709
12.065136	832.902365	11.858727
11.833959	845.258833	11.863744
12.035553	841.298225	11.868762
12.084753	850.940952	11.873779
11.632900	845.842492	11.878797
11.701475	844.796604	11.883815
11.462171	853.029706	11.888832
11.569951	839.834112	11.893850
11.883013	854.292292	11.898867
12.280505	855.779480	11.903885
12.324938	839.851409	11.908903
12.064901	850.176905	11.913920
12.116872	849.796340	11.918938
12.231768	858.434696	11.923955
12.111908	858.036872	11.928973
12.509478	860.010043	11.933991
12.287518	857.024669	11.939008
12.389419	851.747926	11.944026
12.075492	834.771474	11.949043
11.851423	829.391175	11.954061
12.265641	839.039821	11.959079
11.986945	850.617941	11.964096
12.193646	845.084938	11.969114
12.470962	839.487223	11.974131
11.776722	850.107969	11.979149
12.264607	849.103681	11.984167
12.381590	850.581170	11.989184
12.230959	850.052467	11.994202
12.233853	849.023182	11.999219
12.046963	847.282017	12.004237
12.583652	841.179759	12.009255
12.605362	849.252042	12.014272
12.225714	830.660648	12.019290
12.076600	829.339599	12.024307
12.047739	835.482134	12.029325
12.334999	842.111628	12.034343
12.131222	848.429896	12.039360
12.237727	847.924021	12.044378
12.260761	845.985862	12.049395
11.987386	857.058223	12.054413
12.032662	852.036505	12.059431
12.203542	853.805352	12.064448
12.335592	856.306121	12.069466
12.172601	851.152932	12.074483
12.078462	853.089535	12.079501
12.406647	852.561550	12.084519
12.254506	855.479232	12.089536
12.411361	847.953252	12.094554
12.573411	853.939648	12.099571
12.173448	854.425156	12.104589
11.981191	853.603173	12.109607
12.366263	860.510839	12.114624
12.509488	871.284406	12.119642
12.497681	871.166298	12.124659
12.579618	881.703320	12.129677
12.609887	876.179015	12.134695
12.705114	880.515931	12.139712
12.815929	875.764805	12.144730
12.604297	851.696969	12.149747
12.410014	851.724216	12.154765
12.696114	866.224500	12.159783
12.626910	866.412032	12.164800
12.527714	858.402300	12.169818
12.842610	865.459820	12.174835
12.257858	865.807023	12.179853
12.602051	874.128594	12.184871
12.887786	879.117316	12.189888
12.590028	889.338291	12.194906
12.762889	879.572314	12.199923
12.529746	885.828924	12.204941
12.884868	873.787451	12.209959
12.731938	876.042537	12.214976
12.832289	878.560899	12.219994
12.548662	876.951653	12.225011
12.546937	876.730979	12.230029
12.709283	873.376119	12.235047
12.941684	877.050910	12.240064
12.843010	880.373630	12.245082
12.750454	872.100919	12.250099
12.808295	873.212134	12.255117
13.194670	873.997319	12.260135
12.764709	869.709622	12.265152
12.629081	877.478365	12.270170
12.847085	875.910444	12.275187
12.633761	871.658232	12.280205
12.753490	866.684805	12.285223
12.969389	872.101035	12.290240
12.645610	873.117408	12.295258
12.882590	872.010419	12.300275
12.371054	877.651080	12.305293
12.809549	877.907388	12.310311
12.543908	873.830631	12.315328
12.571264	868.795937	12.320346
12.919363	877.631295	12.325363
12.689955	879.298760	12.330381
12.381122	894.917922	12.335399
12.893290	896.355588	12.340416
13.006303	897.022657	12.345434
12.905986	910.248608	12.350451
12.798983	904.408130	12.355469
13.022442	901.425544	12.360487
12.794538	898.166538	12.365504
13.125761	908.528817	12.370522
13.236051	903.547391	12.375539
13.069656	907.868499	12.380557
13.294741	911.452925	12.385575
13.265152	908.487895	12.390592
13.275435	902.281900	12.395610
13.187727	900.424203	12.400627
13.119393	903.780044	12.405645
12.975494	901.842788	12.410663
12.990006	904.358823	12.415680
13.021382	909.851313	12.420698
13.136108	901.438814	12.425715
13.334386	894.723682	12.430733
13.328022	903.778693	12.435751
13.221009	901.586348	12.440768
13.490471	901.136991	12.445786
13.304608	906.515193	12.450803
13.149302	905.731599	12.455821
12.975587	898.658181	12.460839
13.222850	904.621776	12.465856
13.000767	906.789871	12.470874
13.450966	910.850269	12.475891
13.244618	907.262834	12.480909
13.283552	912.151378	12.485927
13.185613	914.110674	12.490944
13.350102	918.420967	12.495962
13.557534	922.314276	12.500979
13.659074	921.600892	12.505997
13.292912	919.354474	12.511015
13.595819	908.245815	12.516032
13.282235	907.543825	12.521050
13.528325	911.797150	12.526067
13.531120	919.181303	12.531085
13.451669	906.999612	12.536103
13.643820	905.281104	12.541120
13.288929	911.114983	12.546138
13.633936	910.877853	12.551155
13.625337	911.387251	12.556173
13.400699	914.183756	12.561191
13.676162	916.564232	12.566208
13.447366	920.314449	12.571226
13.638444	920.316032	12.576243
13.752321	928.326573	12.581261
13.746949	918.115127	12.586279
13.396299	902.447719	12.591296
13.055221	912.239991	12.596314
13.608443	916.612454	12.601331
13.859039	916.125027	12.606349
13.954033	915.914445	12.611367
13.931734	919.815345	12.616384
13.835852	922.247693	12.621402
13.681004	919.586311	12.626419
13.766844	904.393314	12.631437
13.850590	914.513503	12.636455
13.654626	906.484198	12.641472
13.728604	900.609053	12.646490
13.821578	910.093474	12.651507
13.756794	915.951329	12.656525
13.683019	925.493442	12.661543
13.944412	920.911217	12.666560
13.947328	921.971081	12.671578
13.732943	925.387679	12.676595
14.024751	926.127722	12.681613
13.876176	919.564757	12.686631
13.864489	910.562985	12.691648
13.551363	919.508277	12.696666
13.972844	917.198411	12.701683
13.752625	928.335071	12.706701
13.713777	920.199091	12.711719
13.787082	924.526829	12.716736
13.467204	918.060132	12.721754
13.789445	918.754381	12.726771
13.953817	916.257579	12.731789
13.897492	926.323982	12.736807
14.059062	915.773954	12.741824
13.671961	932.462613	12.746842
13.923602	932.445240	12.751859
14.127523	936.212868	12.756877
14.190888	930.544505	12.761895
13.840770	918.294761	12.766912
13.946979	922.541603	12.771930
13.517772	927.626577	12.776947
13.935107	937.770253	12.781965
13.830693	950.864331	12.786983
14.256663	945.552564	12.792000
14.301581	955.331719	12.797018
14.258711	955.347866	12.802035
14.124332	950.054465	12.807053
14.192607	957.507271	12.812071
14.228475	955.295688	12.817088
14.011173	951.741519	12.822106
14.089550	959.369469	12.827123
14.246502	952.187416	12.832141
14.048972	959.558791	12.837159
14.219261	948.751755	12.842176
13.966726	953.455603	12.847194
13.948024	948.775244	12.852211
14.163723	952.462135	12.857229
14.273321	954.625605	12.862247
14.248572	946.462158	12.867264
14.391332	960.514758	12.872282
14.482504	958.026264	12.877299
14.499336	947.473649	12.882317
14.124127	950.511503	12.887335
14.314183	944.343599	12.892352
14.522460	955.403672	12.897370
13.933930	955.293874	12.902387
14.688521	955.996123	12.907405
14.424485	969.938897	12.912423
14.687997	970.935843	12.917440
14.441762	965.600002	12.922458
14.299698	958.922391	12.927475
14.705163	961.866334	12.932493
14.490701	966.715700	12.937511
14.838745	964.250075	12.942528
14.758046	961.390875	12.947546
14.499411	963.249120	12.952563
14.255506	948.132998	12.957581
14.360856	962.529135	12.962599
14.358238	962.813533	12.967616
14.673613	978.309720	12.972634
14.612006	981.547755	12.977651
14.668744	974.943133	12.982669
14.933945	981.099605	12.987687
14.770899	977.546397	12.992704
14.684005	977.900805	12.997722
14.664725	975.123498	13.002739
14.734895	978.467120	13.007757
14.422416	982.271486	13.012775
14.762084	981.833218	13.017792
15.062470	986.548273	13.022810
14.792613	981.187726	13.027827
15.003899	972.573870	13.032845
14.758431	975.626115	13.037863
14.957126	979.817454	13.042880
15.087205	979.541414	13.047898
14.577900	963.529578	13.052915
14.624634	965.516705	13.057933
14.815569	981.704585	13.062951
14.927464	980.023891	13.067968
15.051340	986.391857	13.072986
14.838744	982.918995	13.078003
14.890704	975.308411	13.083021
15.019770	989.647204	13.088039
15.031244	983.728176	13.093056
14.972893	985.895874	13.098074
14.388879	981.764832	13.103091
14.774742	976.645534	13.108109
14.810817	985.223718	13.113127
15.043195	968.890540	13.118144
14.605098	975.318150	13.123162
14.902289	976.073131	13.128179
15.101843	978.651704	13.133197
14.982927	986.818667	13.138215
15.004975	982.479057	13.143232
15.242087	980.472628	13.148250
14.747547	978.997404	13.153267
14.936390	974.723182	13.158285
15.194477	981.878012	13.163303
15.074561	972.410324	13.168320
15.187342	975.040361	13.173338
15.172067	967.134198	13.178355
15.158740	960.666793	13.183373
14.902089	975.735046	13.188391
14.985967	995.196533	13.193408
15.503435	1002.051953	13.198426
15.229926	1005.168557	13.203443
15.772348	1000.210918	13.208461
15.049351	1004.619258	13.213479
15.295049	994.936481	13.218496
15.459557	1003.055889	13.223514
15.176729	1000.588117	13.228531
15.387203	990.396460	13.233549
15.303265	999.031324	13.238567
15.520497	998.905732	13.243584
15.645076	1004.721323	13.248602
15.552033	992.191406	13.253619
15.547344	973.250776	13.258637
15.341108	981.598678	13.263655
15.434032	974.432959	13.268672
15.345476	980.244066	13.273690
15.306530	978.706928	13.278707
15.611283	972.770355	13.283725
15.701489	992.593769	13.288743
15.242449	978.483326	13.293760
15.501850	991.438380	13.298778
15.432909	992.484259	13.303795
15.871846	994.005992	13.308813
15.573986	993.964260	13.313831
15.711194	976.976949	13.318848
15.512120	970.466059	13.323866
15.538805	982.782220	13.328883
15.899460	984.761190	13.333901
15.283882	980.051264	13.338919
15.524044	989.124498	13.343936
15.720809	989.601722	13.348954
15.576030	993.367192	13.353971
15.707901	991.749640	13.358989
15.551906	994.686882	13.364007
15.587857	994.018487	13.369024
15.763184	991.488400	13.374042
15.377853	988.197238	13.379059
15.698699	987.954425	13.384077
15.389279	992.361079	13.389095
15.734026	993.077052	13.394112
15.457365	989.585824	13.399130
15.252051	1001.212505	13.404147
15.930672	1001.175571	13.409165
16.106402	1018.113799	13.414183
15.927456	1016.481827	13.419200
15.854657	1007.637906	13.424218
16.066309	1022.090020	13.429235
15.991857	1005.987922	13.434253
15.852901	1008.991926	13.439271
16.067434	1013.840362	13.444288
15.777780	1009.656882	13.449306
15.951521	1012.435166	13.454323
16.068041	1015.377052	13.459341
16.230594	1013.000444	13.464359
16.089039	1004.877362	13.469376
16.168357	1000.487748	13.474394
15.738549	995.773958	13.479411
16.018237	1016.706968	13.484429
16.067727	1017.235670	13.489447
16.273410	1022.072872	13.494464
16.388937	1025.933266	13.499482
15.825275	1010.005645	13.504499
16.046044	1018.920984	13.509517
15.902019	1015.203841	13.514535
15.895038	1023.252295	13.519552
16.406647	1019.852153	13.524570
15.899026	1024.365609	13.529587
16.343215	1017.091188	13.534605
16.552310	1019.478921	13.539623
16.458515	1021.576436	13.544640
16.504727	1015.431046	13.549658
16.154349	1028.872992	13.554675
16.254197	1028.027324	13.559693
16.571743	1028.409884	13.564711
16.373094	1026.064621	13.569728
16.194366	1017.167864	13.574746
16.107313	1023.493152	13.579763
16.377837	1022.529223	13.584781
16.210076	1018.481279	13.589799
16.067016	1020.621227	13.594816
16.346234	1025.210219	13.599834
16.061582	1028.628379	13.604851
16.410087	1018.418235	13.609869
16.180631	1016.011528	13.614887
16.242977	1022.625835	13.619904
16.554111	1012.787628	13.624922
16.354109	1023.069103	13.629939
16.457583	1018.066622	13.634957
16.554394	1033.963180	13.639975
16.525762	1037.085604	13.644992
16.493711	1038.936759	13.650010
16.674087	1055.227347	13.655027
16.624900	1043.441614	13.660045
16.914645	1043.090063	13.665063
16.780630	1044.745752	13.670080
16.790980	1024.429919	13.675098
16.912164	1025.086245	13.680115
16.994939	1009.622237	13.685133
16.593365	1012.351804	13.690151
16.307878	1018.932246	13.695168
16.725185	1003.428451	13.700186
16.843592	1022.338598	13.705203
16.848565	1014.268293	13.710221
16.774491	1014.589135	13.715239
16.603621	1017.292024	13.720256
16.851599	1025.461481	13.725274
16.870511	1047.880762	13.730291
16.785440	1045.441961	13.735309
16.757128	1048.349740	13.740327
16.760680	1043.230362	13.745344
17.024351	1036.448127	13.750362
16.624919	1045.561640	13.755379
17.043176	1043.204925	13.760397
17.114557	1038.898598	13.765415
16.811887	1047.088068	13.770432
16.977790	1041.321552	13.775450
16.879530	1045.199667	13.780467
16.730057	1041.600137	13.785485
17.140295	1035.328276	13.790503
16.596825	1047.408761	13.795520
16.788932	1042.584894	13.800538
16.472851	1038.648547	13.805555
16.484842	1037.671475	13.810573
17.039439	1044.117145	13.815591
17.132041	1073.341543	13.820608
17.329242	1060.892336	13.825626
17.016305	1066.031716	13.830643
17.252865	1061.614295	13.835661
17.411843	1065.644617	13.840679
17.307274	1059.945720	13.845696
17.277757	1056.087548	13.850714
17.147113	1045.772579	13.855731
16.928258	1052.465671	13.860749
17.478470	1055.519496	13.865767
17.200986	1068.072724	13.870784
17.663838	1055.597677	13.875802
17.194103	1054.115405	13.880819
17.300768	1056.175205	13.885837
17.394823	1054.645624	13.890855
17.416793	1071.055721	13.895872
17.558616	1051.776468	13.900890
17.351489	1046.109423	13.905907
17.214656	1055.749849	13.910925
17.601216	1056.714897	13.915943
17.058944	1053.378883	13.920960
17.664864	1058.336425	13.925978
17.580052	1066.261392	13.930995
17.247084	1062.485478	13.936013
17.546773	1060.920522	13.941031
17.208113	1064.154644	13.946048
17.807335	1054.552146	13.951066
17.811132	1058.332222	13.956083
17.466306	1055.224052	13.961101
17.502386	1067.422033	13.966119
17.111437	1065.864298	13.971136
17.450939	1063.311635	13.976154
17.377408	1066.494748	13.981171
17.267170	1065.199150	13.986189
17.521557	1059.166297	13.991207
17.659074	1062.688733	13.996224
17.918375	1060.593610	14.001242
17.907288	1059.143620	14.006259
17.921530	1064.547322	14.011277
17.755494	1062.061243	14.016295
17.405517	1067.973299	14.021312
17.433569	1061.123828	14.026330
17.613252	1067.918587	14.031347
17.591376	1087.084314	14.036365
17.973432	1081.056698	14.041383
17.818966	1079.651261	14.046400
17.923334	1087.265726	14.051418
17.971397	1093.531998	14.056435
17.826118	1091.358248	14.061453
18.173081	1090.319222	14.066471
17.679484	1093.239948	14.071488
17.885266	1092.226198	14.076506
18.125762	1091.781375	14.081523
18.044399	1090.355016	14.086541
18.370347	1092.932737	14.091559
17.608943	1091.546654	14.096576
18.017105	1085.057347	14.101594
17.919436	1080.922665	14.106611
18.302989	1086.839720	14.111629
18.222622	1074.670682	14.116647
18.426903	1075.380264	14.121664
17.870083	1076.379511	14.126682
17.880490	1077.823224	14.131699
18.089366	1082.571577	14.136717
18.133802	1075.498624	14.141735
18.041402	1081.632263	14.146752
18.170590	1079.835239	14.151770
18.507185	1084.595141	14.156787
18.700364	1084.994033	14.161805
18.550680	1078.506923	14.166823
18.109696	1084.714115	14.171840
18.203990	1085.481956	14.176858
18.283167	1087.138960	14.181875
18.114041	1080.588623	14.186893
18.895311	1077.584883	14.191911
18.102739	1089.341503	14.196928
18.147593	1088.898930	14.201946
18.364587	1091.178136	14.206963
18.177617	1091.399901	14.211981
18.358728	1082.535096	14.216999
18.325386	1085.046031	14.222016
18.132368	1093.095263	14.227034
18.325209	1092.143502	14.232051
18.129858	1090.880172	14.237069
18.298902	1095.906174	14.242087
18.472819	1116.155273	14.247104
18.422452	1111.315728	14.252122
18.660231	1114.812998	14.257139
18.669376	1117.181579	14.262157
18.716347	1114.106687	14.267175
18.639972	1113.799875	14.272192
18.698438	1117.079083	14.277210
18.760829	1114.749714	14.282227
18.635782	1112.979898	14.287245
18.427674	1114.287434	14.292263
18.603938	1117.573433	14.297280
18.642390	1118.198543	14.302298
18.631803	1110.092763	14.307315
18.692094	1117.723615	14.312333
18.818093	1118.464398	14.317351
18.676120	1115.652644	14.322368
18.946563	1108.563202	14.327386
19.153293	1111.311085	14.332403
18.579769	1118.930788	14.337421
18.999143	1115.737587	14.342439
18.715222	1124.514300	14.347456
18.893104	1107.810831	14.352474
19.249426	1110.573147	14.357491
19.186936	1113.227511	14.362509
18.986249	1112.283757	14.367527
18.983381	1117.762742	14.372544
18.986320	1107.038636	14.377562
18.763120	1110.254675	14.382579
18.746313	1112.453749	14.387597
19.039154	1107.197508	14.392615
18.713003	1112.190647	14.397632
18.629302	1109.142541	14.402650
18.944032	1119.008902	14.407667
18.693485	1131.889319	14.412685
19.226534	1138.227945	14.417703
19.305671	1132.923127	14.422720
19.377060	1134.792799	14.427738
19.723763	1132.573519	14.432755
19.300303	1135.312846	14.437773
19.575914	1132.612390	14.442791
19.422155	1129.897155	14.447808
19.311120	1115.681584	14.452826
19.467300	1114.533591	14.457843
19.167704	1114.006129	14.462861
19.404489	1109.569725	14.467879
19.399815	1110.763335	14.472896
19.184762	1110.702317	14.477914
19.294272	1118.704160	14.482931
19.215588	1129.844017	14.487949
19.566668	1131.461580	14.492967
19.647419	1132.212610	14.497984
19.253043	1130.456587	14.503002
19.391550	1125.814668	14.508019
19.222120	1132.247576	14.513037
19.441213	1130.332318	14.518055
19.500545	1131.238185	14.523072
19.554377	1131.835639	14.528090
19.344764	1131.350883	14.533107
19.109272	1143.250633	14.538125
19.432405	1125.000108	14.543143
19.178176	1133.507081	14.548160
19.208033	1134.890946	14.553178
19.657375	1140.160226	14.558195
20.021958	1154.787306	14.563213
19.655616	1150.420144	14.568231
19.854486	1138.052674	14.573248
19.732103	1137.674174	14.578266
19.830227	1127.796693	14.583283
19.816730	1119.640871	14.588301
19.676013	1132.882784	14.593319
19.851527	1139.056518	14.598336
19.994088	1144.553751	14.603354
19.775688	1137.206368	14.608371
19.676874	1145.818386	14.613389
19.989083	1155.180223	14.618407
20.207107	1156.897532	14.623424
19.977287	1144.007079	14.628442
20.101066	1140.970642	14.633459
19.719050	1145.010004	14.638477
20.116881	1154.282685	14.643495
20.412205	1142.998341	14.648512
20.099452	1142.318302	14.653530
20.085907	1124.653868	14.658547
19.731280	1131.857421	14.663565
20.006952	1126.796372	14.668583
20.516137	1139.469396	14.673600
20.155419	1137.509280	14.678618
20.165395	1126.585241	14.683635
20.238193	1131.077212	14.688653
20.112909	1124.551548	14.693671
19.908993	1132.091256	14.698688
19.781807	1144.734600	14.703706
20.316730	1146.477997	14.708723
20.143937	1146.296746	14.713741
20.224205	1146.520823	14.718759
20.604209	1152.608873	14.723776
20.489388	1150.764865	14.728794
20.858396	1154.090100	14.733811
20.403497	1151.731320	14.738829
20.221153	1144.084789	14.743847
20.690023	1149.250025	14.748864
20.343773	1141.616553	14.753882
20.011395	1148.387428	14.758899
20.160334	1154.041458	14.763917
20.583729	1155.830733	14.768935
20.445589	1152.926852	14.773952
20.320451	1152.081715	14.778970
20.440845	1152.936989	14.783987
20.323184	1152.185356	14.789005
20.295865	1148.197430	14.794023
20.554430	1144.808509	14.799040
20.340168	1148.389234	14.804058
20.404121	1146.779154	14.809075
20.359971	1156.392489	14.814093
20.654744	1166.378770	14.819111
21.057430	1161.143173	14.824128
20.575167	1163.787574	14.829146
20.599461	1155.275512	14.834163
20.497171	1157.500609	14.839181
20.645474	1175.522591	14.844199
21.008334	1171.192654	14.849216
20.668251	1176.724491	14.854234
21.135972	1171.387181	14.859251
20.956108	1166.246012	14.864269
20.878000	1164.815982	14.869287
20.847792	1146.652355	14.874304
20.483532	1167.036327	14.879322
20.825178	1160.743610	14.884339
20.884469	1175.819336	14.889357
21.081850	1179.663782	14.894375
21.496540	1173.362773	14.899392
20.794036	1187.213465	14.904410
21.025556	1177.946231	14.909427
21.000153	1173.434124	14.914445
21.115661	1176.486651	14.919463
21.476671	1174.788999	14.924480
21.312500	1173.369296	14.929498
21.398419	1155.035984	14.934515
20.994711	1146.540492	14.939533
20.699759	1153.684210	14.944551
20.919630	1164.300775	14.949568
20.771437	1168.057349	14.954586
20.982421	1169.450708	14.959603
21.064363	1174.865928	14.964621
21.242112	1170.596553	14.969639
21.231004	1172.387634	14.974656
21.138173	1167.857690	14.979674
21.373402	1160.243559	14.984691
20.959329	1174.399352	14.989709
21.344809	1174.553517	14.994727
21.256562	1172.272990	14.999744
21.391516	1187.863901	15.004762
21.479422	1180.496911	15.009779
21.521940	1200.842434	15.014797
21.544795	1193.182667	15.019815
21.865158	1193.391217	15.024832
21.390298	1166.287223	15.029850
21.545305	1160.979977	15.034867
21.759841	1165.727466	15.039885
21.142622	1165.114065	15.044903
21.657953	1178.947514	15.049920
21.994412	1184.846733	15.054938
22.088201	1177.983762	15.059955
21.774881	1171.497009	15.064973
21.479694	1170.145172	15.069991
21.607724	1163.197945	15.075008
21.408072	1162.206688	15.080026
21.566275	1175.796282	15.085043
21.798608	1191.368783	15.090061
21.671566	1194.970567	15.095079
21.709475	1181.744642	15.100096
21.363910	1189.170864	15.105114
21.883447	1190.004630	15.110131
21.621297	1184.040042	15.115149
21.777713	1194.802270	15.120167
21.869316	1187.403138	15.125184
21.842113	1196.736124	15.130202
21.759802	1185.678182	15.135219
21.896705	1182.112652	15.140237
21.472631	1188.951559	15.145255
22.092045	1181.782164	15.150272
21.959241	1189.866188	15.155290
21.892830	1200.145768	15.160307
22.162088	1202.584061	15.165325
21.858793	1219.581756	15.170343
22.335911	1212.740764	15.175360
22.590556	1216.983354	15.180378
22.744216	1201.353435	15.185395
22.206729	1187.457093	15.190413
22.277376	1186.117365	15.195431
22.347393	1180.381608	15.200448
22.210403	1190.542850	15.205466
22.167257	1182.890272	15.210483
22.241164	1191.995970	15.215501
22.028726	1186.377050	15.220519
22.230930	1175.242979	15.225536
22.269384	1177.253518	15.230554
21.893278	1179.067073	15.235571
22.050889	1194.269424	15.240589
22.297235	1202.518115	15.245607
22.519102	1204.556725	15.250624
22.435289	1210.158876	15.255642
22.895936	1213.643338	15.260659
22.483410	1210.185977	15.265677
21.918690	1214.796792	15.270695
22.214170	1213.235638	15.275712
22.265634	1207.578520	15.280730
22.142507	1198.868625	15.285747
22.347761	1205.217607	15.290765
22.111422	1218.269434	15.295783
22.431926	1227.696283	15.300800
22.798865	1228.765403	15.305818
22.857336	1238.119701	15.310835
23.032272	1233.399461	15.315853
22.768416	1226.362127	15.320871
23.075878	1228.690295	15.325888
23.191554	1234.396900	15.330906
23.149175	1210.377802	15.335923
22.796656	1208.656239	15.340941
22.742531	1208.450083	15.345959
22.658680	1203.136067	15.350976
22.756834	1191.920455	15.355994
23.013499	1200.126501	15.361011
22.811085	1205.295943	15.366029
22.639297	1224.763024	15.371047
22.970871	1232.537616	15.376064
23.250249	1228.397475	15.381082
23.205820	1231.954764	15.386099
23.363333	1227.827405	15.391117
23.129010	1214.543120	15.396135
22.982295	1207.124514	15.401152
22.671827	1217.230900	15.406170
23.013486	1228.633170	15.411187
23.296926	1231.627836	15.416205
23.419877	1243.165371	15.421223
23.278974	1234.685467	15.426240
23.496652	1234.114825	15.431258
23.281864	1230.418191	15.436275
23.385829	1228.281114	15.441293
23.193839	1236.292378	15.446311
23.572761	1217.559636	15.451328
23.392137	1209.666649	15.456346
23.013353	1212.455792	15.461363
23.249206	1217.364061	15.466381
23.049481	1229.106782	15.471399
23.778446	1224.261869	15.476416
23.719836	1231.636837	15.481434
23.226061	1229.120031	15.486451
23.618750	1236.739880	15.491469
23.533863	1238.621425	15.496487
23.689746	1236.154313	15.501504
23.541865	1240.671420	15.506522
23.166423	1242.538528	15.511539
23.255471	1242.385680	15.516557
22.852357	1245.497385	15.521575
23.332773	1235.588350	15.526592
23.611320	1226.389464	15.531610
23.657901	1231.993282	15.536627
23.609758	1231.240221	15.541645
23.683988	1237.780162	15.546663
23.768035	1236.425707	15.551680
23.706081	1243.125845	15.556698
23.647688	1253.375797	15.561715
24.158976	1250.764633	15.566733
23.969829	1261.943971	15.571751
24.154404	1239.441971	15.576768
23.906073	1231.442814	15.581786
23.417834	1230.765019	15.586803
24.035222	1245.160056	15.591821
24.090937	1256.932202	15.596839
24.142225	1244.906526	15.601856
24.158703	1238.797276	15.606874
23.906753	1233.449626	15.611891
23.807777	1233.203159	15.616909
24.459205	1249.306509	15.621927
24.369323	1244.637225	15.626944
24.123478	1233.481796	15.631962
23.668630	1233.884392	15.636979
24.375807	1243.809257	15.641997
24.178202	1250.562211	15.647015
24.102049	1249.488482	15.652032
24.285125	1252.924921	15.657050
24.586450	1257.393742	15.662067
24.445807	1252.981724	15.667085
24.472199	1259.163085	15.672103
24.263472	1245.903170	15.677120
24.397393	1242.757827	15.682138
24.436968	1239.860802	15.687155
24.456538	1252.856779	15.692173
24.270952	1263.527462	15.697191
24.533734	1260.358771	15.702208
24.189783	1253.447587	15.707226
24.238662	1251.148721	15.712243
24.274487	1252.762039	15.717261
24.098484	1246.935415	15.722279
24.013069	1247.952332	15.727296
24.239167	1247.295161	15.732314
24.200532	1263.699151	15.737331
24.460017	1271.497680	15.742349
24.303774	1271.821932	15.747367
24.336446	1270.993090	15.752384
24.197127	1274.710425	15.757402
24.572206	1279.887239	15.762419
24.741678	1265.608663	15.767437
24.513627	1277.340074	15.772455
24.590570	1272.906584	15.777472
25.035991	1283.803470	15.782490
25.000619	1299.976602	15.787507
25.269747	1286.357756	15.792525
25.065425	1280.718600	15.797543
25.053297	1267.904405	15.802560
25.080537	1263.854254	15.807578
25.043226	1267.044352	15.812595
25.344025	1270.541247	15.817613
24.640958	1274.602536	15.822631
24.838191	1271.816508	15.827648
25.042317	1273.169923	15.832666
24.784127	1277.524437	15.837683
24.916626	1279.996792	15.842701
24.972886	1292.068685	15.847719
25.254315	1292.901892	15.852736
25.411835	1299.968463	15.857754
25.064119	1303.999330	15.862771
25.350035	1291.911614	15.867789
25.151119	1305.339503	15.872807
25.290073	1288.073905	15.877824
25.651715	1291.318267	15.882842
25.694019	1291.819701	15.887859
25.515013	1284.100001	15.892877
25.154964	1287.293330	15.897895
25.349804	1292.387932	15.902912
25.824512	1294.440588	15.907930
25.291054	1283.885628	15.912947
25.309042	1284.999958	15.917965
25.558030	1277.408868	15.922983
25.153646	1287.959208	15.928000
25.199163	1287.797401	15.933018
25.232984	1290.218945	15.938035
25.270857	1282.294847	15.943053
25.293821	1285.301931	15.948071
25.271201	1286.747679	15.953088
25.613420	1294.479605	15.958106
25.608755	1312.301624	15.963123
26.059348	1316.062245	15.968141
25.465827	1312.093564	15.973159
25.620072	1316.320350	15.978176
26.144179	1303.343215	15.983194
25.784244	1317.616874	15.988211
26.031792	1316.107405	15.993229
26.003883	1320.340640	15.998247
25.946379	1314.192462	16.003264
25.959350	1311.896057	16.008282
25.675075	1306.313602	16.013299
25.725921	1315.981570	16.018317
26.177794	1313.660581	16.023335
26.212503	1320.493930	16.028352
26.123879	1297.621239	16.033370
26.032259	1314.033577	16.038387
25.999679	1312.350241	16.043405
26.028166	1319.143538	16.048423
25.752376	1314.519143	16.053440
26.064027	1309.973128	16.058458
26.310443	1315.211138	16.063475
26.042955	1319.270465	16.068493
26.052367	1318.543098	16.073511
25.937864	1314.881228	16.078528
25.991108	1305.667107	16.083546
26.090152	1325.540000	16.088563
26.523173	1339.796737	16.093581
26.444492	1334.598640	16.098599
26.361556	1337.057418	16.103616
26.683354	1331.105433	16.108634
26.734871	1338.365358	16.113651
26.218294	1331.923017	16.118669
26.613904	1330.513428	16.123687
26.475711	1327.814660	16.128704
26.621511	1324.175122	16.133722
26.947580	1337.107358	16.138739
26.768125	1328.469343	16.143757
26.725441	1324.799374	16.148775
26.433377	1320.600418	16.153792
26.811666	1328.118418	16.158810
26.628793	1337.201304	16.163827
26.576036	1330.733630	16.168845
26.746051	1335.649092	16.173863
26.867362	1337.132255	16.178880
26.739999	1335.287038	16.183898
26.446377	1334.525095	16.188915
26.547357	1335.159352	16.193933
26.782582	1337.918586	16.198951
26.593911	1329.146311	16.203968
26.987297	1332.505632	16.208986
26.504334	1336.305225	16.214003
26.449895	1330.001922	16.219021
26.875225	1339.260923	16.224039
26.981292	1346.474434	16.229056
27.293091	1346.971515	16.234074
27.031849	1356.890380	16.239091
27.288892	1353.896146	16.244109
27.193553	1364.085676	16.249127
27.423172	1351.059969	16.254144
27.349599	1354.744929	16.259162
27.455139	1346.261074	16.264179
27.132288	1346.011811	16.269197
26.968539	1330.933299	16.274215
27.285451	1344.892642	16.279232
27.806775	1345.599900	16.284250
27.598952	1352.187230	16.289267
27.486871	1337.917995	16.294285
27.285455	1327.636042	16.299303
27.558960	1340.803742	16.304320
27.579849	1330.995056	16.309338
27.340015	1341.955161	16.314355
27.490771	1346.867331	16.319373
27.400333	1343.946477	16.324391
27.678121	1354.737123	16.329408
27.867870	1344.195051	16.334426
27.230958	1345.153210	16.339443
27.495703	1348.415921	16.344461
27.491614	1349.186564	16.349479
27.702132	1350.141341	16.354496
27.978278	1344.262778	16.359514
27.911407	1345.213676	16.364531
27.900394	1346.708106	16.369549
27.643717	1337.037583	16.374567
27.309177	1341.492440	16.379584
27.245644	1335.449344	16.384602
27.412410	1342.700681	16.389619
27.482237	1353.782694	16.394637
27.851632	1363.833135	16.399655
27.891993	1363.631109	16.404672
28.490953	1361.665777	16.409690
28.135476	1369.361878	16.414707
27.552677	1372.855219	16.419725
27.685096	1365.888290	16.424743
28.551359	1375.665223	16.429760
28.387657	1372.547554	16.434778
27.771931	1370.396984	16.439795
27.920983	1374.343722	16.444813
28.241367	1363.115276	16.449831
28.224689	1374.018344	16.454848
28.417473	1369.787593	16.459866
28.254442	1370.021390	16.464883
28.061771	1366.684191	16.469901
28.386584	1363.673025	16.474919
28.114217	1370.655495	16.479936
28.505242	1371.061266	16.484954
28.515730	1385.576753	16.489971
28.705881	1385.436467	16.494989
28.520340	1373.280547	16.500007
28.653301	1372.915685	16.505024
28.693401	1370.141637	16.510042
28.748772	1367.346261	16.515059
28.532510	1369.895363	16.520077
28.697054	1368.787071	16.525095
28.610052	1371.265427	16.530112
28.599525	1372.002365	16.535130
28.726729	1368.211092	16.540147
28.450093	1368.150253	16.545165
28.869342	1378.801982	16.550183
28.682730	1397.387919	16.555200
28.767613	1392.763801	16.560218
28.755489	1390.184131	16.565235
28.829291	1390.649073	16.570253
28.967274	1391.444797	16.575271
28.889206	1400.385058	16.580288
28.899733	1385.582161	16.585306
29.014016	1389.493324	16.590323
29.164166	1392.205934	16.595341
29.189735	1394.379467	16.600359
29.197737	1393.696501	16.605376
29.175423	1384.819236	16.610394
29.093261	1393.198383	16.615411
28.976310	1391.013846	16.620429
29.381697	1391.938093	16.625447
28.884075	1393.029069	16.630464
28.996514	1388.356451	16.635482
28.960531	1384.515001	16.640499
28.988449	1390.740352	16.645517
29.381795	1387.895175	16.650535
29.280901	1394.787670	16.655552
29.222671	1387.740146	16.660570
29.251388	1393.009132	16.665587
29.480777	1403.390811	16.670605
29.599153	1411.599687	16.675623
29.476132	1416.327546	16.680640
29.606724	1417.499983	16.685658
29.645166	1421.991099	16.690675
28.975020	1419.296765	16.695693
29.698447	1418.211361	16.700711
29.688111	1422.407152	16.705728
29.780676	1413.410885	16.710746
29.772124	1409.236917	16.715763
29.462260	1413.523818	16.720781
29.630218	1408.151352	16.725799
29.545991	1410.200074	16.730816
29.628852	1405.674102	16.735834
29.636231	1409.759814	16.740851
29.518562	1415.840720	16.745869
29.676095	1411.577611	16.750887
29.878347	1432.163468	16.755904
29.795650	1425.709919	16.760922
30.236952	1426.303482	16.765939
29.961009	1438.512733	16.770957
30.321828	1433.283617	16.775975
30.186731	1431.430133	16.780992
30.010067	1427.020560	16.786010
30.548103	1439.136993	16.791027
30.484497	1437.720448	16.796045
30.534064	1416.334481	16.801063
30.163004	1408.556452	16.806080
30.017992	1401.882294	16.811098
30.089117	1410.796028	16.816115
30.448054	1427.579705	16.821133
30.511094	1423.000028	16.826151
30.656205	1424.801374	16.831168
30.306299	1423.054133	16.836186
30.255160	1418.151507	16.841203
30.462865	1425.377528	16.846221
30.662339	1423.029798	16.851239
30.693406	1425.518065	16.856256
30.656381	1429.736975	16.861274
30.614983	1426.054160	16.866291
30.371238	1429.033625	16.871309
30.786658	1422.382108	16.876327
30.698343	1429.512495	16.881344
30.793265	1428.503473	16.886362
30.944545	1425.222830	16.891379
30.845900	1425.588555	16.896397
30.889598	1416.366405	16.901415
30.728957	1407.229925	16.906432
30.408868	1421.932940	16.911450
30.717714	1423.759126	16.916467
30.878547	1429.010579	16.921485
30.588813	1424.514576	16.926503
30.827328	1423.369443	16.931520
30.333526	1433.141744	16.936538
30.746749	1420.320759	16.941555
30.900102	1425.699619	16.946573
31.057909	1434.975338	16.951591
31.127693	1443.371729	16.956608
30.981100	1448.074886	16.961626
31.320367	1446.472138	16.966643
31.191242	1448.890830	16.971661
31.063198	1447.762101	16.976679
30.694780	1448.037545	16.981696
31.072821	1444.970688	16.986714
31.090408	1447.634646	16.991731
31.189936	1451.819543	16.996749
31.643158	1450.880618	17.001767
31.337936	1445.345584	17.006784
31.138453	1446.342513	17.011802
31.744799	1451.820826	17.016819
31.416192	1453.251411	17.021837
31.550372	1444.261232	17.026855
31.519100	1447.857529	17.031872
31.141662	1457.207654	17.036890
31.644147	1456.450365	17.041907
31.515479	1470.015700	17.046925
31.899090	1478.113619	17.051943
31.913579	1473.421611	17.056960
31.871872	1470.783446	17.061978
31.910385	1460.088270	17.066995
32.002378	1471.873809	17.072013
32.252012	1464.074249	17.077031
31.894309	1459.134434	17.082048
31.701771	1465.769906	17.087066
32.017433	1461.223224	17.092083
31.944415	1477.134162	17.097101
32.114449	1461.533010	17.102119
32.225049	1472.599241	17.107136
32.111236	1470.859187	17.112154
32.089690	1472.718209	17.117171
31.746017	1479.841285	17.122189
32.004350	1472.785156	17.127207
31.864066	1473.084820	17.132224
32.091331	1473.636177	17.137242
32.172968	1462.274656	17.142259
31.842066	1479.819740	17.147277
32.318871	1468.320559	17.152295
31.977072	1476.178670	17.157312
32.255360	1486.729468	17.162330
32.448717	1492.351399	17.167347
31.946724	1493.417818	17.172365
32.285991	1496.299637	17.177383
32.584596	1496.098175	17.182400
32.636137	1501.177417	17.187418
32.528408	1492.603826	17.192435
32.800918	1488.890752	17.197453
32.697856	1489.869420	17.202471
32.571231	1490.596149	17.207488
32.387194	1498.795640	17.212506
32.974047	1489.911246	17.217523
32.487442	1499.149103	17.222541
32.594417	1480.865809	17.227559
32.243755	1479.983404	17.232576
32.278590	1491.478099	17.237594
32.969927	1501.348785	17.242611
32.709491	1509.639149	17.247629
32.908894	1515.547329	17.252647
33.088348	1513.227971	17.257664
32.785040	1513.142906	17.262682
33.324641	1510.300044	17.267699
33.164824	1515.731154	17.272717
32.746020	1512.726015	17.277735
33.413462	1508.603907	17.282752
33.165839	1518.372398	17.287770
33.584636	1514.797350	17.292787
33.210082	1513.994429	17.297805
33.342053	1509.426021	17.302823
33.465047	1513.528357	17.307840
33.344256	1522.219742	17.312858
33.000183	1511.464553	17.317875
33.220570	1513.396131	17.322893
32.957755	1507.876524	17.327911
33.305078	1500.945302	17.332928
33.020866	1500.551121	17.337946
32.758210	1516.270891	17.342963
33.188785	1532.781500	17.347981
33.080061	1530.680868	17.352999
33.752026	1530.319918	17.358016
33.312546	1538.464771	17.363034
33.615799	1537.079105	17.368051
33.602382	1537.939584	17.373069
34.034160	1551.196255	17.378087
33.951429	1540.965014	17.383104
33.650255	1537.142990	17.388122
33.742959	1543.560222	17.393139
34.227981	1549.145941	17.398157
34.318907	1546.206106	17.403175
34.583876	1533.995272	17.408192
33.989825	1533.166777	17.413210
34.032374	1521.337952	17.418227
33.853220	1525.209909	17.423245
33.700532	1520.329478	17.428263
34.320672	1531.315911	17.433280
34.035254	1545.069970	17.438298
34.595414	1545.083159	17.443315
34.269619	1540.132010	17.448333
34.175233	1523.865304	17.453351
34.355514	1523.947478	17.458368
33.983823	1531.182267	17.463386
34.498769	1539.455305	17.468403
34.703895	1548.433324	17.473421
34.659093	1550.595811	17.478439
34.492368	1540.601802	17.483456
34.238454	1540.218652	17.488474
34.858341	1548.942331	17.493491
34.476622	1547.951175	17.498509
34.237747	1561.991457	17.503527
34.357446	1553.154976	17.508544
34.345400	1552.020690	17.513562
34.554645	1547.531687	17.518579
34.806526	1556.802199	17.523597
34.599169	1545.154530	17.528615
34.683126	1551.352221	17.533632
34.519332	1553.848945	17.538650
35.040730	1550.393520	17.543667
34.958563	1553.335066	17.548685
34.775449	1554.667121	17.553703
35.020378	1551.056189	17.558720
34.824048	1551.929548	17.563738
34.940514	1541.130588	17.568755
35.042196	1554.243312	17.573773
35.250605	1569.355969	17.578791
35.377345	1562.661264	17.583808
34.756715	1565.684021	17.588826
35.157800	1565.633767	17.593843
35.542726	1569.729793	17.598861
34.996146	1571.061989	17.603879
35.188030	1566.616729	17.608896
35.016763	1575.413883	17.613914
35.135932	1575.322588	17.618931
35.609431	1573.228562	17.623949
35.483828	1567.103590	17.628967
35.461916	1569.906305	17.633984
35.436400	1576.503025	17.639002
35.440071	1564.421476	17.644019
35.452322	1561.112096	17.649037
35.399602	1566.731578	17.654055
35.458627	1562.821553	17.659072
35.416562	1571.033548	17.664090
35.788677	1573.114936	17.669107
35.816373	1590.244167	17.674125
35.373400	1584.768543	17.679143
36.019860	1588.375453	17.684160
35.986150	1590.974883	17.689178
36.130270	1584.949662	17.694195
36.050567	1587.976038	17.699213
35.930833	1585.801381	17.704231
36.275488	1576.427849	17.709248
35.945356	1587.721001	17.714266
36.316087	1591.825568	17.719283
36.254312	1586.315465	17.724301
35.799788	1579.714981	17.729319
36.040441	1575.268390	17.734336
36.095379	1580.599598	17.739354
36.218131	1584.761951	17.744371
36.072500	1581.452057	17.749389
36.180222	1580.564102	17.754407
36.569705	1580.247411	17.759424
36.597943	1592.983490	17.764442
36.381021	1587.762794	17.769459
36.346053	1583.488778	17.774477
36.270012	1587.729618	17.779495
36.433432	1584.828913	17.784512
36.330778	1580.294092	17.789530
36.250910	1579.274576	17.794547
36.514268	1590.247515	17.799565
36.411688	1599.863932	17.804583
36.222608	1607.149038	17.809600
36.213999	1613.332850	17.814618
36.537888	1610.915106	17.819635
36.657320	1608.914423	17.824653
36.779305	1608.847934	17.829671
36.825637	1607.275289	17.834688
36.912222	1619.210102	17.839706
36.816195	1629.807008	17.844723
37.253583	1628.337200	17.849741
37.347042	1638.049161	17.854759
37.343256	1618.792111	17.859776
36.992697	1615.552189	17.864794
37.213249	1620.257831	17.869811
37.415372	1609.637922	17.874829
36.952977	1606.715339	17.879847
37.394229	1618.648235	17.884864
37.486688	1617.021022	17.889882
37.156093	1611.736075	17.894899
37.506384	1607.849836	17.899917
37.364525	1611.719124	17.904935
37.539893	1617.792058	17.909952
37.784133	1612.685302	17.914970
37.366821	1613.612222	17.919987
37.559924	1610.467011	17.925005
37.135226	1610.372561	17.930023
37.278552	1619.915745	17.935040
37.430721	1632.903847	17.940058
37.767396	1627.116699	17.945075
37.953635	1622.760676	17.950093
37.649690	1632.471779	17.955111
37.831119	1625.036302	17.960128
37.765772	1628.483333	17.965146
37.561964	1629.471481	17.970163
37.786906	1621.129742	17.975181
37.433383	1635.554134	17.980199
37.475404	1630.864082	17.985216
37.760948	1648.369555	17.990234
37.713741	1651.072099	17.995251
38.282639	1654.334552	18.000269
38.107145	1660.162656	18.005287
38.029337	1659.824499	18.010304
38.196115	1652.880479	18.015322
38.062060	1650.957378	18.020339
38.578728	1658.583231	18.025357
38.284103	1656.694755	18.030375
38.115461	1650.633305	18.035392
37.975680	1648.423910	18.040410
37.969066	1658.192587	18.045427
38.238862	1662.698011	18.050445
38.426764	1676.573682	18.055463
38.308418	1670.337078	18.060480
38.802142	1672.415205	18.065498
38.718691	1671.838079	18.070515
39.111389	1668.942466	18.075533
38.651290	1682.869172	18.080551
38.876013	1672.406640	18.085568
38.707267	1671.353704	18.090586
38.703474	1674.093633	18.095603
38.988575	1664.530560	18.100621
39.092883	1675.279151	18.105639
38.810299	1670.756718	18.110656
39.044477	1675.318221	18.115674
38.875681	1683.010454	18.120691
39.238589	1669.048406	18.125709
38.982838	1672.115003	18.130727
39.184500	1668.823266	18.135744
39.216321	1662.765119	18.140762
39.266648	1671.022647	18.145779
39.497391	1661.647983	18.150797
39.238032	1675.985067	18.155815
39.270785	1673.291022	18.160832
39.133787	1671.276857	18.165850
39.300325	1671.216012	18.170867
39.424520	1669.722685	18.175885
39.181856	1673.825541	18.180903
38.990851	1671.295949	18.185920
39.030330	1686.312090	18.190938
39.297229	1696.719623	18.195955
39.636472	1686.015066	18.200973
39.126979	1698.096975	18.205991
39.586995	1693.426628	18.211008
39.733289	1693.409982	18.216026
39.487977	1696.512819	18.221043
39.827240	1689.399742	18.226061
39.496990	1691.313464	18.231079
39.860835	1704.079095	18.236096
39.559300	1710.564468	18.241114
39.956166	1716.624823	18.246131
40.143238	1716.797458	18.251149
40.051858	1714.574159	18.256167
40.317191	1717.552809	18.261184
40.238034	1714.039961	18.266202
40.155556	1720.266943	18.271219
40.495123	1709.877918	18.276237
40.451402	1716.919377	18.281255
40.286322	1717.390195	18.286272
40.641294	1720.799793	18.291290
40.184590	1698.691195	18.296307
40.176884	1704.133245	18.301325
40.491845	1719.267206	18.306343
40.257882	1713.862942	18.311360
40.656225	1716.012825	18.316378
40.103987	1707.821216	18.321395
40.415217	1714.409410	18.326413
40.444290	1720.675722	18.331431
40.487586	1710.557189	18.336448
40.637903	1706.869526	18.341466
40.288835	1715.041321	18.346483
40.528559	1715.666477	18.351501
40.695043	1733.111788	18.356519
40.848093	1734.204985	18.361536
41.070864	1730.531213	18.366554
40.729305	1738.518796	18.371571
40.849065	1740.346238	18.376589
41.073476	1738.196541	18.381607
40.837253	1738.485993	18.386624
41.179657	1734.698798	18.391642
40.846189	1738.134206	18.396659
41.496133	1731.502639	18.401677
41.314676	1736.870931	18.406695
41.077143	1734.335996	18.411712
41.404998	1723.790999	18.416730
41.100491	1726.290858	18.421747
41.113422	1729.946561	18.426765
41.402060	1738.394013	18.431783
41.300158	1744.942799	18.436800
41.379329	1749.086771	18.441818
40.962597	1761.962118	18.446835
41.390512	1750.110636	18.451853
41.488533	1751.130400	18.456871
41.569150	1748.861213	18.461888
41.780586	1748.117956	18.466906
41.338206	1754.126768	18.471923
41.147757	1756.564577	18.476941
42.046349	1770.215356	18.481959
41.813066	1781.269381	18.486976
42.085782	1767.779003	18.491994
42.099239	1772.835886	18.497011
42.500956	1775.714278	18.502029
42.244631	1774.798141	18.507047
42.284957	1769.978924	18.512064
42.497477	1756.289692	18.517082
41.986417	1755.694349	18.522099
42.227223	1755.760730	18.527117
42.360325	1763.456193	18.532135
42.253345	1765.966137	18.537152
42.338988	1769.973393	18.542170
42.814338	1771.682006	18.547187
42.590241	1756.786168	18.552205
42.397160	1746.767769	18.557223
42.109040	1752.241144	18.562240
42.456315	1766.357016	18.567258
42.509763	1768.696650	18.572275
42.714278	1764.508152	18.577293
43.054527	1770.160807	18.582311
42.681262	1764.289177	18.587328
42.911600	1764.802191	18.592346
42.753636	1769.605048	18.597363
42.880771	1767.038221	18.602381
43.078277	1768.118142	18.607399
42.739883	1771.475430	18.612416
42.840550	1767.205367	18.617434
42.785869	1766.923548	18.622451
42.756589	1761.089547	18.627469
43.103551	1770.285309	18.632487
42.728262	1766.752572	18.637504
42.716123	1761.105244	18.642522
42.945628	1763.818102	18.647539
42.846823	1771.748730	18.652557
43.076449	1785.318129	18.657575
43.271389	1791.744681	18.662592
43.370775	1788.115478	18.667610
43.163202	1799.399028	18.672627
43.476476	1787.821117	18.677645
43.756028	1785.741675	18.682663
43.201752	1790.786522	18.687680
43.486624	1788.311749	18.692698
43.411444	1791.037632	18.697715
43.450466	1789.466116	18.702733
43.554745	1792.485793	18.707751
43.495018	1805.178997	18.712768
44.027024	1812.146070	18.717786
43.885066	1818.338221	18.722803
44.054883	1822.294429	18.727821
43.953919	1814.477060	18.732839
43.975932	1817.575906	18.737856
44.077259	1809.212420	18.742874
43.811222	1808.932154	18.747891
43.985257	1813.095995	18.752909
44.314616	1810.652120	18.757927
44.191429	1813.237197	18.762944
44.255638	1816.253688	18.767962
44.056886	1819.601729	18.772979
44.055210	1817.575814	18.777997
44.090553	1813.757812	18.783015
43.712107	1825.926578	18.788032
44.431847	1824.964815	18.793050
44.272046	1837.815741	18.798067
44.225920	1840.486584	18.803085
44.444585	1836.283228	18.808103
44.698213	1839.099622	18.813120
44.723303	1839.887807	18.818138
44.450464	1840.082005	18.823155
44.619612	1844.202434	18.828173
44.909730	1835.187627	18.833191
44.454827	1842.217814	18.838208
45.048641	1860.574653	18.843226
45.237310	1862.044151	18.848243
44.641687	1863.652311	18.853261
44.704545	1867.663159	18.858279
44.726402	1862.537523	18.863296
45.013262	1863.240512	18.868314
45.272302	1862.597095	18.873331
45.097115	1855.419380	18.878349
45.380327	1855.949360	18.883367
44.857458	1863.056480	18.888384
45.174078	1855.678626	18.893402
45.166837	1857.096763	18.898419
45.342343	1872.407347	18.903437
45.808382	1873.438890	18.908455
45.561321	1875.008219	18.913472
45.642989	1866.370059	18.918490
45.702492	1856.921130	18.923507
45.452560	1860.498117	18.928525
45.660591	1868.068270	18.933543
46.021381	1891.558578	18.938560
45.998879	1870.139177	18.943578
45.895991	1863.713881	18.948595
46.083666	1862.371548	18.953613
46.074441	1849.935200	18.958631
45.582661	1855.797142	18.963648
45.952218	1869.117450	18.968666
46.311227	1881.123372	18.973683
46.253122	1869.013424	18.978701
46.398073	1864.221973	18.983719
45.991096	1861.088681	18.988736
46.143100	1864.921450	18.993754
46.165990	1870.324041	18.998771
46.204323	1871.413128	19.003789
46.294441	1867.113134	19.008807
46.023545	1874.411167	19.013824
46.394954	1871.970164	19.018842
46.586048	1877.235944	19.023859
46.513002	1871.209937	19.028877
46.648050	1868.509304	19.033895
46.246781	1871.141114	19.038912
46.248347	1862.629122	19.043930
46.616780	1875.959080	19.048947
46.515793	1896.785498	19.053965
46.755197	1889.741640	19.058983
46.489958	1903.972523	19.064000
47.101049	1897.287019	19.069018
46.982478	1904.510703	19.074035
47.223869	1897.655890	19.079053
46.900221	1899.679060	19.084071
46.841549	1901.187314	19.089088
46.872089	1898.973294	19.094106
47.342971	1894.275945	19.099123
46.995023	1899.114915	19.104141
47.042786	1900.341390	19.109159
47.112621	1917.079300	19.114176
47.408696	1921.343972	19.119194
47.285908	1916.616548	19.124211
47.131944	1925.471125	19.129229
47.558863	1919.161629	19.134247
47.372614	1923.965804	19.139264
47.426139	1918.043034	19.144282
47.822205	1914.209522	19.149299
47.873085	1919.554091	19.154317
47.774672	1916.448188	19.159335
47.629897	1911.834670	19.164352
47.502861	1911.015041	19.169370
47.753123	1922.384736	19.174387
47.661108	1940.419894	19.179405
47.965478	1937.276129	19.184423
47.626610	1944.016759	19.189440
48.255268	1937.527316	19.194458
48.476232	1932.364153	19.199475
47.910528	1936.438782	19.204493
48.261357	1938.880178	19.209511
48.113160	1940.787495	19.214528
47.812377	1934.642503	19.219546
47.980043	1932.555326	19.224563
48.544815	1950.856844	19.229581
48.599333	1956.822587	19.234599
48.448053	1960.093785	19.239616
48.482756	1955.209123	19.244634
48.618008	1943.460175	19.249651
48.474839	1955.055645	19.254669
49.059533	1947.815645	19.259687
48.877955	1948.396358	19.264704
48.836745	1957.135449	19.269722
49.239968	1952.335070	19.274739
49.198524	1955.778418	19.279757
49.255100	1934.469635	19.284775
48.682938	1926.161118	19.289792
48.703898	1930.301629	19.294810
49.375052	1942.454358	19.299827
48.710473	1951.856039	19.304845
49.202788	1945.495260	19.309863
49.117848	1937.426002	19.314880
48.740998	1948.303795	19.319898
49.180426	1954.335471	19.324915
49.087315	1945.642600	19.329933
49.163765	1943.601274	19.334951
49.067581	1957.275503	19.339968
49.150141	1962.971750	19.344986
49.336827	1972.259004	19.350003
49.281427	1978.428181	19.355021
49.565315	1973.031071	19.360039
49.766796	1980.902119	19.365056
49.591564	1975.939882	19.370074
49.313206	1973.499677	19.375091
49.547741	1989.754228	19.380109
49.933392	1997.476500	19.385127
49.979971	1990.292389	19.390144
50.073277	2001.711974	19.395162
50.225877	2003.187136	19.400179
49.946029	2010.234145	19.405197
50.190484	1994.485162	19.410215
50.225222	1998.389985	19.415232
49.934378	2002.030218	19.420250
50.146247	1987.845417	19.425267
49.932753	1997.081767	19.430285
50.192504	1994.175372	19.435303
50.661124	2000.849473	19.440320
50.111921	2006.591064	19.445338
50.286323	2013.235523	19.450355
50.750444	2019.193920	19.455373
50.574343	2010.738097	19.460391
50.741273	2019.731806	19.465408
50.407368	2019.525290	19.470426
50.996536	2021.386521	19.475443
50.537696	2021.530962	19.480461
50.799653	2014.429869	19.485479
50.686494	2014.346569	19.490496
50.775685	2015.853759	19.495514
50.957464	2021.831145	19.500531
51.085762	2037.654230	19.505549
51.229507	2036.350327	19.510567
51.183210	2037.973427	19.515584
51.306353	2039.345902	19.520602
51.233951	2034.162397	19.525619
51.478047	2037.703044	19.530637
51.527529	2033.784944	19.535655
51.537442	2036.541717	19.540672
51.404822	2043.575140	19.545690
51.622783	2029.698643	19.550707
51.683193	2036.367282	19.555725
51.620352	2037.781520	19.560743
51.886603	2036.928671	19.565760
51.534726	2038.722732	19.570778
51.407965	2036.280859	19.575795
51.310470	2028.027322	19.580813
51.547531	2048.734677	19.585831
51.847234	2053.229202	19.590848
51.937619	2055.231704	19.595866
52.284566	2053.712914	19.600883
51.953683	2060.581733	19.605901
52.270078	2059.121381	19.610919
52.630740	2051.626086	19.615936
52.150237	2051.013319	19.620954
52.405494	2050.591411	19.625971
52.260738	2060.445072	19.630989
52.275883	2051.776217	19.636007
52.713064	2051.007047	19.641024
52.368636	2049.640763	19.646042
52.506122	2056.906446	19.651059
52.356880	2056.415360	19.656077
52.472721	2065.991493	19.661095
52.948787	2052.554255	19.666112
52.558810	2056.585597	19.671130
52.572861	2053.092795	19.676147
52.407349	2076.709990	19.681165
52.834970	2074.891359	19.686183
52.916040	2074.607202	19.691200
52.791965	2079.063981	19.696218
52.957923	2071.864290	19.701235
53.349399	2078.515791	19.706253
53.098926	2078.564465	19.711271
53.183159	2075.048039	19.716288
52.682689	2067.409926	19.721306
53.167544	2074.921015	19.726323
53.312906	2093.973250	19.731341
53.125090	2101.791727	19.736359
53.215928	2095.525357	19.741376
53.107103	2101.819720	19.746394
53.323825	2097.146360	19.751411
53.546925	2093.807003	19.756429
53.901780	2102.837586	19.761447
54.053429	2110.277811	19.766464
53.866690	2117.007294	19.771482
54.146530	2111.714926	19.776499
54.001611	2108.871915	19.781517
53.926562	2101.722596	19.786535
54.234347	2098.278445	19.791552
54.332387	2119.765111	19.796570
54.427899	2097.001414	19.801587
54.082523	2106.170113	19.806605
54.261313	2108.954090	19.811623
54.369808	2111.345109	19.816640
54.507015	2119.813311	19.821658
54.886184	2115.332261	19.826675
54.642233	2113.006575	19.831693
54.086932	2100.826036	19.836711
54.730418	2110.723496	19.841728
54.481153	2124.147261	19.846746
54.805931	2119.589519	19.851763
54.273478	2125.426360	19.856781
54.534762	2132.060406	19.861799
54.991511	2125.676732	19.866816
54.622227	2115.635236	19.871834
54.632711	2115.542032	19.876851
54.800500	2118.236209	19.881869
54.740103	2132.050143	19.886887
55.120830	2140.783180	19.891904
55.300337	2146.189721	19.896922
55.022126	2149.414563	19.901939
55.107594	2152.396219	19.906957
55.081968	2148.855962	19.911975
55.401994	2143.557289	19.916992
55.354609	2142.018216	19.922010
55.392905	2143.186226	19.927027
55.295481	2141.402510	19.932045
55.308652	2145.007764	19.937063
55.755199	2148.892284	19.942080
55.678596	2154.559876	19.947098
55.715242	2162.229595	19.952115
55.723455	2162.408165	19.957133
55.811875	2163.969141	19.962151
55.709360	2163.723214	19.967168
55.410064	2156.287091	19.972186
55.710800	2161.930282	19.977203
55.838307	2161.411613	19.982221
56.178768	2173.307020	19.987239
56.192469	2178.518625	19.992256
56.554039	2186.617165	19.997274
56.610156	2185.333293	20.002291
56.781285	2170.574019	20.007309
56.176377	2160.260121	20.012327
56.123206	2158.340073	20.017344
56.067845	2168.482767	20.022362
56.246199	2178.225904	20.027379
56.622238	2177.983900	20.032397
56.299163	2181.818582	20.037415
56.753039	2177.240599	20.042432
56.558750	2176.867028	20.047450
56.672196	2184.726711	20.052467
57.071471	2198.421335	20.057485
56.998424	2199.966583	20.062503
57.248189	2198.267332	20.067520
57.131794	2207.636910	20.072538
57.444607	2202.471904	20.077555
57.174272	2197.622344	20.082573
57.450031	2199.542166	20.087591
57.446998	2203.642314	20.092608
57.224755	2197.380776	20.097626
57.466926	2195.184059	20.102643
57.336004	2200.522479	20.107661
57.736331	2203.044526	20.112679
57.574068	2196.035076	20.117696
57.456755	2203.504854	20.122714
57.502684	2194.209365	20.127731
57.542628	2193.682322	20.132749
57.662020	2197.548676	20.137767
58.202826	2192.976006	20.142784
57.897571	2217.940821	20.147802
57.886214	2215.316727	20.152819
58.114387	2222.012804	20.157837
58.218974	2227.743557	20.162855
58.611777	2223.651695	20.167872
58.248864	2234.259212	20.172890
58.264447	2228.130829	20.177907
58.373516	2212.409179	20.182925
57.983377	2218.984361	20.187943
58.384896	2220.512067	20.192960
58.271754	2217.610407	20.197978
58.233099	2216.114145	20.202995
58.360694	2206.670144	20.208013
58.447873	2215.092577	20.213031
58.816355	2229.546346	20.218048
58.709681	2229.824975	20.223066
58.887981	2236.585680	20.228083
59.011752	2234.577936	20.233101
59.114184	2233.839113	20.238119
59.294880	2223.215887	20.243136
58.914368	2233.264383	20.248154
59.037593	2241.422384	20.253171
59.188501	2230.286227	20.258189
59.143709	2237.754126	20.263207
59.131742	2229.092589	20.268224
59.113463	2225.478577	20.273242
59.000403	2234.257464	20.278259
59.698974	2245.228896	20.283277
59.518515	2259.775008	20.288295
59.654492	2256.089480	20.293312
59.711169	2266.495566	20.298330
59.795275	2264.307825	20.303347
59.822550	2255.820022	20.308365
59.762935	2261.021046	20.313383
60.186456	2250.571215	20.318400
60.125050	2264.050866	20.323418
59.627635	2256.667833	20.328435
59.332347	2248.994338	20.333453
59.337053	2257.256129	20.338471
60.117000	2274.214501	20.343488
60.291311	2276.361682	20.348506
60.242454	2279.897780	20.353523
60.367803	2271.748083	20.358541
60.154239	2279.501239	20.363559
60.239320	2275.470202	20.368576
60.286974	2273.398634	20.373594
60.169072	2279.053799	20.378611
60.419414	2287.204529	20.383629
60.232266	2297.835042	20.388647
60.692010	2293.600122	20.393664
60.516773	2294.391308	20.398682
60.882084	2302.495627	20.403699
61.111693	2291.384976	20.408717
61.049197	2290.713020	20.413735
61.377757	2296.651721	20.418752
61.245362	2306.317372	20.423770
61.427009	2313.434218	20.428787
61.377386	2303.134232	20.433805
61.272186	2295.124797	20.438823
61.759773	2301.379439	20.443840
61.948349	2310.221568	20.448858
61.713333	2313.487012	20.453875
61.976295	2294.159039	20.458893
61.384147	2287.428361	20.463911
61.293367	2289.108950	20.468928
61.587483	2298.512098	20.473946
61.361529	2308.413333	20.478963
61.850427	2310.981484	20.483981
61.736962	2313.524081	20.488999
61.917480	2308.171471	20.494016
61.645862	2317.827380	20.499034
62.123778	2325.390160	20.504051
62.086736	2332.190952	20.509069
61.995055	2335.992568	20.514087
62.263154	2334.460860	20.519104
62.356725	2326.473921	20.524122
61.934866	2334.461723	20.529139
62.406616	2329.918775	20.534157
62.499397	2340.372900	20.539175
62.696639	2351.628088	20.544192
62.730584	2362.782625	20.549210
62.350697	2363.350236	20.554227
62.932306	2355.321538	20.559245
62.621282	2364.380835	20.564263
62.651938	2363.435484	20.569280
62.930120	2364.152478	20.574298
62.539032	2361.720412	20.579315
63.259432	2370.791699	20.584333
63.190296	2378.809472	20.589351
63.041363	2385.795087	20.594368
63.245699	2390.336201	20.599386
63.373589	2389.167312	20.604403
63.559958	2379.373156	20.609421
63.494788	2380.099760	20.614439
63.639773	2377.296500	20.619456
63.796679	2374.343036	20.624474
64.116699	2377.947602	20.629491
63.820207	2364.448120	20.634509
63.924263	2374.982557	20.639527
64.065438	2372.328230	20.644544
64.225085	2378.943576	20.649562
63.968157	2379.491922	20.654579
63.788312	2375.830603	20.659597
64.033728	2377.938251	20.664615
63.804005	2363.888619	20.669632
63.932738	2373.630169	20.674650
63.698199	2379.350981	20.679667
64.037031	2384.180317	20.684685
63.897700	2392.878184	20.689703
64.025905	2394.069997	20.694720
64.313721	2390.786724	20.699738
64.470732	2418.257912	20.704755
64.750775	2424.545115	20.709773
64.675573	2423.562692	20.714791
64.607745	2423.626936	20.719808
64.754748	2430.449427	20.724826
64.856680	2429.436096	20.729843
64.918431	2421.693963	20.734861
65.049894	2426.615766	20.739879
64.892467	2420.274561	20.744896
64.826701	2434.253684	20.749914
65.314217	2441.098576	20.754931
65.374982	2445.466521	20.759949
65.315467	2441.499131	20.764967
65.380459	2447.018387	20.769984
65.559327	2450.629302	20.775002
65.246891	2441.692818	20.780019
65.523901	2448.498103	20.785037
65.528267	2456.479146	20.790055
65.525333	2466.465458	20.795072
65.818705	2468.830716	20.800090
65.802709	2471.001424	20.805107
66.137421	2474.045079	20.810125
66.032710	2472.417120	20.815143
65.728592	2474.484634	20.820160
65.823776	2469.678727	20.825178
66.083924	2475.520899	20.830195
66.078969	2480.691329	20.835213
66.165518	2489.312823	20.840231
66.582661	2489.086470	20.845248
66.226793	2482.798426	20.850266
66.083311	2496.060714	20.855283
66.754867	2489.819999	20.860301
66.586381	2485.102740	20.865319
66.609165	2494.990356	20.870336
66.644152	2505.128553	20.875354
66.734435	2522.185746	20.880371
66.882133	2500.937761	20.885389
67.004888	2513.460851	20.890407
67.199320	2516.258222	20.895424
67.265351	2515.218949	20.900442
67.597379	2514.990150	20.905459
67.532199	2514.239704	20.910477
67.529670	2515.092212	20.915495
67.353771	2520.074821	20.920512
67.887020	2509.430907	20.925530
67.397771	2512.464794	20.930547
67.596829	2505.262900	20.935565
67.457005	2506.297879	20.940583
67.705650	2514.553130	20.945600
67.996487	2524.663878	20.950618
67.900977	2534.942469	20.955635
68.195776	2526.990193	20.960653
68.317659	2528.984657	20.965671
68.129141	2534.016588	20.970688
68.351555	2530.481580	20.975706
68.170026	2535.304114	20.980723
68.299708	2526.929540	20.985741
68.374919	2527.062900	20.990759
68.247710	2536.914072	20.995776
68.435377	2529.442528	21.000794
67.959122	2529.857968	21.005811
68.011208	2525.863606	21.010829
68.553137	2538.103268	21.015847
68.291360	2549.190632	21.020864
68.586284	2552.410964	21.025882
68.512163	2559.296554	21.030899
68.759691	2561.034628	21.035917
68.594242	2560.271485	21.040935
68.873081	2573.249891	21.045952
68.906373	2569.807628	21.050970
68.918530	2574.268434	21.055987
69.146381	2576.404107	21.061005
69.481769	2576.613481	21.066023
69.324705	2580.640009	21.071040
69.642822	2580.277675	21.076058
69.111018	2582.276722	21.081075
69.375840	2593.723466	21.086093
69.724255	2594.991256	21.091111
69.578852	2597.788229	21.096128
70.122838	2598.769732	21.101146
69.774290	2599.389250	21.106163
69.902667	2597.361807	21.111181
70.324839	2589.017125	21.116199
70.186288	2601.590684	21.121216
70.081360	2588.010523	21.126234
70.290276	2605.178609	21.131251
70.554228	2614.100605	21.136269
70.526551	2616.898074	21.141287
70.394271	2628.028321	21.146304
70.675637	2621.015477	21.151322
70.645309	2622.282642	21.156339
70.608835	2616.099160	21.161357
70.671054	2614.893204	21.166375
70.493739	2621.955948	21.171392
70.881744	2608.835083	21.176410
70.827942	2611.368373	21.181427
71.036260	2622.050738	21.186445
71.136872	2625.393055	21.191463
70.921192	2643.861746	21.196480
71.228224	2643.261283	21.201498
71.184175	2650.625084	21.206515
71.269807	2646.142552	21.211533
71.213386	2643.560173	21.216551
71.300112	2650.979232	21.221568
71.840440	2657.153146	21.226586
71.628642	2666.790401	21.231603
71.707251	2668.775880	21.236621
71.849454	2674.750217	21.241639
71.832492	2673.301016	21.246656
72.391464	2669.621723	21.251674
71.887037	2669.044241	21.256691
71.879271	2661.158247	21.261709
72.031564	2667.872692	21.266727
71.652130	2668.670637	21.271744
72.199341	2672.394319	21.276762
72.158914	2687.669996	21.281779
72.260662	2688.313650	21.286797
72.224061	2683.768200	21.291815
72.261484	2686.688038	21.296832
72.284236	2680.845586	21.301850
72.661493	2700.007314	21.306867
72.469810	2708.798751	21.311885
73.027476	2703.569992	21.316903
72.818455	2710.640894	21.321920
73.260490	2705.916296	21.326938
72.970754	2714.631570	21.331955
73.079993	2710.754458	21.336973
72.961561	2708.169161	21.341991
73.142402	2713.291612	21.347008
72.962091	2712.571820	21.352026
73.135799	2737.616964	21.357043
73.358363	2726.642863	21.362061
73.562771	2727.753324	21.367079
73.599360	2735.865157	21.372096
73.377419	2731.307703	21.377114
73.458020	2738.383738	21.382131
73.795471	2749.213223	21.387149
73.597124	2759.160877	21.392167
73.497004	2754.959913	21.397184
73.921751	2757.809610	21.402202
74.208743	2769.761133	21.407219
74.433747	2778.566224	21.412237
74.606416	2778.046774	21.417255
74.771103	2783.032905	21.422272
74.934936	2777.345063	21.427290
74.830342	2782.303948	21.432307
75.034957	2769.874490	21.437325
75.110213	2755.088728	21.442343
74.727371	2761.195853	21.447360
74.907523	2750.515591	21.452378
74.720427	2754.717294	21.457395
74.883034	2767.385812	21.462413
75.163036	2773.038758	21.467431
74.890991	2772.090312	21.472448
74.896135	2778.730012	21.477466
75.479910	2774.453456	21.482483
75.404322	2778.075899	21.487501
75.763799	2766.954077	21.492519
75.223283	2778.018973	21.497536
75.551900	2789.976613	21.502554
75.621213	2795.507924	21.507571
75.637044	2792.727991	21.512589
75.548520	2799.167755	21.517607
75.727122	2808.027472	21.522624
75.396606	2805.648977	21.527642
75.705056	2809.056607	21.532659
75.649213	2823.889796	21.537677
76.158621	2834.184249	21.542695
76.281173	2834.849899	21.547712
76.097479	2836.194761	21.552730
76.356150	2834.882264	21.557747
76.383785	2847.559361	21.562765
77.157118	2847.469725	21.567783
76.912632	2850.316979	21.572800
76.740285	2856.504778	21.577818
76.927876	2848.240917	21.582835
76.851443	2860.063225	21.587853
77.194081	2843.452265	21.592871
76.904832	2855.453097	21.597888
76.944253	2852.991387	21.602906
76.979816	2850.880617	21.607923
77.199513	2853.014444	21.612941
77.297239	2858.718068	21.617959
77.456465	2865.131665	21.622976
77.569277	2863.933547	21.627994
77.884481	2867.182321	21.633011
77.771840	2882.788250	21.638029
77.869601	2871.451717	21.643047
77.735724	2865.273942	21.648064
77.540643	2867.081391	21.653082
77.578475	2854.242455	21.658099
77.598133	2863.449031	21.663117
78.106177	2855.987124	21.668135
78.145450	2864.922354	21.673152
78.147165	2887.173040	21.678170
78.275278	2896.574104	21.683187
78.498372	2894.266671	21.688205
78.534783	2881.494217	21.693223
78.376829	2897.104101	21.698240
78.238884	2888.174773	21.703258
78.662725	2889.336082	21.708275
78.614526	2890.479819	21.713293
79.061886	2889.756365	21.718311
78.637687	2913.131130	21.723328
78.814899	2912.393190	21.728346
78.972668	2912.756644	21.733363
78.929349	2915.455612	21.738381
79.108113	2902.007512	21.743399
78.987703	2919.808232	21.748416
79.222770	2928.138393	21.753434
79.581587	2932.655442	21.758451
79.386182	2931.903287	21.763469
79.660563	2931.200621	21.768487
79.352982	2931.719044	21.773504
79.690283	2938.385667	21.778522
79.532348	2941.361403	21.783539
79.422368	2950.575709	21.788557
79.760909	2952.201721	21.793575
79.812417	2950.650241	21.798592
79.993980	2968.217482	21.803610
80.231052	2979.479449	21.808627
80.148670	2986.546399	21.813645
80.931183	2981.897790	21.818663
80.650512	2976.197466	21.823680
80.698617	2982.199273	21.828698
80.688327	2985.123478	21.833715
80.700726	2985.579146	21.838733
81.034760	2975.729970	21.843751
81.238522	2985.406441	21.848768
80.833466	2983.721337	21.853786
80.775045	2976.275539	21.858803
80.945891	2998.521958	21.863821
81.272018	2996.908512	21.868839
81.251439	3000.023703	21.873856
81.339142	3000.587508	21.878874
81.457937	2999.489442	21.883891
81.410341	3001.987097	21.888909
81.845563	3013.811405	21.893927
81.544313	3037.204942	21.898944
81.718090	3030.426574	21.903962
81.817847	3028.444598	21.908979
81.595599	3029.820765	21.913997
81.755605	3020.377573	21.919015
81.619255	3036.965770	21.924032
82.080837	3047.839111	21.929050
82.280173	3050.572674	21.934067
82.127872	3043.343554	21.939085
81.991174	3038.744260	21.944103
82.469963	3068.896139	21.949120
82.577334	3077.199032	21.954138
82.675605	3073.812773	21.959155
82.827204	3083.642656	21.964173
82.510028	3069.502018	21.969191
82.808623	3075.565609	21.974208
82.921586	3076.526297	21.979226
82.966569	3087.707960	21.984243
83.088242	3094.304269	21.989261
83.384153	3095.810725	21.994279
83.650252	3097.700597	21.999296
83.617904	3097.667754	22.004314
83.586958	3080.420742	22.009331
83.656314	3101.029336	22.014349
83.805193	3091.963440	22.019367
83.930980	3097.164062	22.024384
83.920842	3092.207212	22.029402
83.899849	3090.171555	22.034419
83.713331	3100.351103	22.039437
83.914043	3095.746275	22.044455
84.037935	3102.496894	22.049472
84.066526	3108.782703	22.054490
84.110127	3117.070356	22.059507
84.024787	3118.522922	22.064525
84.303233	3120.698077	22.069543
84.581657	3121.743312	22.074560
84.770078	3137.772569	22.079578
84.808035	3146.354648	22.084595
84.966201	3144.335102	22.089613
84.755992	3138.595281	22.094631
84.878699	3142.060481	22.099648
84.828379	3146.588029	22.104666
85.250876	3145.451842	22.109683
85.094958	3157.299422	22.114701
85.376837	3153.786539	22.119719
85.460577	3157.797561	22.124736
85.646821	3160.463755	22.129754
85.749841	3164.342353	22.134771
85.639314	3168.986651	22.139789
85.893417	3162.852143	22.144807
85.983661	3153.214657	22.149824
85.938325	3161.759294	22.154842
85.867687	3161.558857	22.159859
85.983677	3186.569482	22.164877
86.186697	3188.241998	22.169895
86.481614	3185.875932	22.174912
86.093586	3187.685236	22.179930
86.218119	3184.083375	22.184947
86.132445	3198.583830	22.189965
86.472082	3203.804635	22.194983
86.679519	3204.756841	22.200000
86.586227	3208.981827	22.205018
86.935794	3208.008561	22.210035
86.782842	3212.533268	22.215053
87.027649	3218.056151	22.220071
87.229861	3223.481554	22.225088
87.228699	3236.864118	22.230106
87.320284	3228.602500	22.235123
87.218058	3234.788911	22.240141
87.567914	3240.497342	22.245159
87.654325	3230.096608	22.250176
87.728689	3235.889230	22.255194
87.972608	3234.863077	22.260211
87.717422	3250.223376	22.265229
87.969980	3266.611979	22.270247
88.141913	3259.799096	22.275264
87.873009	3263.739141	22.280282
88.338365	3268.056522	22.285299
88.201712	3260.477676	22.290317
87.898176	3255.118563	22.295335
88.309175	3268.663826	22.300352
88.043713	3290.805369	22.305370
88.436396	3281.208807	22.310387
88.826135	3289.028842	22.315405
88.627004	3283.542894	22.320423
88.963740	3279.844643	22.325440
88.640739	3296.228759	22.330458
89.158640	3294.411648	22.335475
89.248271	3296.464908	22.340493
89.311868	3301.056709	22.345511
89.446111	3301.414390	22.350528
89.396280	3298.452135	22.355546
89.552950	3301.246078	22.360563
89.664218	3298.346958	22.365581
89.802893	3298.808100	22.370599
89.599467	3292.196044	22.375616
89.640174	3302.005544	22.380634
89.572695	3304.449543	22.385651
89.811454	3318.125985	22.390669
90.100063	3321.555759	22.395687
89.998488	3323.875697	22.400704
89.795224	3327.931721	22.405722
90.131494	3340.649185	22.410739
90.269426	3344.733820	22.415757
90.248185	3353.012803	22.420775
90.752156	3355.155810	22.425792
90.486811	3357.094253	22.430810
90.658654	3368.290933	22.435827
91.416794	3371.378873	22.440845
90.888005	3372.241277	22.445863
91.015721	3367.830880	22.450880
91.053265	3389.303289	22.455898
91.269825	3379.172454	22.460915
91.425158	3387.417476	22.465933
91.594889	3392.273580	22.470951
91.950147	3401.926541	22.475968
91.649041	3402.156742	22.480986
91.645915	3398.865215	22.486003
91.799008	3398.781224	22.491021
91.716901	3401.445310	22.496039
92.156776	3393.018580	22.501056
92.278305	3404.077977	22.506074
91.970805	3400.550073	22.511091
91.865908	3412.500296	22.516109
92.004339	3418.683785	22.521127
92.254410	3415.721869	22.526144
92.286909	3434.048328	22.531162
92.372070	3438.532629	22.536179
92.990138	3446.692556	22.541197
92.707705	3446.720987	22.546215
92.992369	3443.744178	22.551232
92.842202	3443.865512	22.556250
93.221320	3454.799364	22.561267
93.427904	3466.546166	22.566285
93.077495	3471.120811	22.571303
93.185435	3465.807637	22.576320
93.543971	3472.540571	22.581338
93.611050	3468.890842	22.586355
93.335920	3475.445301	22.591373
93.853852	3493.875675	22.596391
93.953772	3488.058747	22.601408
94.100745	3501.178422	22.606426
94.222951	3502.775254	22.611443
93.845522	3497.872680	22.616461
94.276796	3497.262195	22.621479
94.445747	3488.524364	22.626496
94.405784	3494.751610	22.631514
94.504579	3513.815800	22.636531
95.051247	3514.809564	22.641549
94.905817	3510.789117	22.646567
95.119714	3508.341015	22.651584
94.938015	3509.287922	22.656602
94.915094	3508.650752	22.661619
94.986575	3513.490718	22.666637
94.918846	3516.004223	22.671655
95.202535	3503.457716	22.676672
94.844627	3518.218862	22.681690
95.153819	3535.151185	22.686707
95.234388	3535.586717	22.691725
95.258500	3539.944888	22.696743
95.455983	3543.852956	22.701760
95.600890	3565.270878	22.706778
95.640456	3569.358350	22.711795
95.579087	3573.136539	22.716813
95.842041	3576.333660	22.721831
95.995597	3576.293784	22.726848
96.004171	3590.805037	22.731866
96.342408	3584.133261	22.736883
96.380444	3589.786499	22.741901
95.865997	3594.175403	22.746919
96.302484	3601.297021	22.751936
96.488486	3615.464867	22.756954
96.640638	3612.786546	22.761971
97.163865	3621.819925	22.766989
97.211715	3640.191532	22.772007
97.404946	3634.031683	22.777024
97.650020	3631.790152	22.782042
97.527088	3633.475902	22.787059
97.901702	3630.166184	22.792077
97.412459	3640.822721	22.797095
97.571516	3634.156905	22.802112
97.645556	3634.202081	22.807130
97.789567	3635.533536	22.812147
97.831551	3626.992283	22.817165
97.790370	3649.531540	22.822183
97.863488	3659.213060	22.827200
97.917520	3660.949995	22.832218
98.049011	3658.820945	22.837235
98.705027	3675.989444	22.842253
98.206895	3687.338632	22.847271
98.611730	3674.081795	22.852288
98.589890	3683.453106	22.857306
98.826189	3689.583479	22.862323
98.663661	3684.205301	22.867341
98.903707	3703.657882	22.872359
99.009627	3709.865503	22.877376
99.084033	3707.789579	22.882394
99.187145	3707.549289	22.887411
99.153565	3715.953467	22.892429
99.516087	3730.964892	22.897447
99.831140	3733.096512	22.902464
99.906838	3742.209535	22.907482
99.739700	3744.022161	22.912499
99.789515	3731.029221	22.917517
99.760509	3737.864003	22.922535
100.362763	3742.368369	22.927552
100.563508	3752.784305	22.932570
100.502787	3754.409818	22.937587
100.306182	3750.356302	22.942605
100.278585	3754.801535	22.947623
100.363824	3752.518748	22.952640
100.384869	3752.231345	22.957658
100.992271	3772.276648	22.962675
100.997467	3769.526638	22.967693
100.952318	3773.526426	22.972711
100.893256	3774.394163	22.977728
101.594916	3772.352526	22.982746
101.170375	3775.815209	22.987763
101.341084	3782.896475	22.992781
101.271370	3782.329752	22.997799
101.466746	3799.109713	23.002816
101.699320	3804.050772	23.007834
101.623008	3806.325781	23.012851
101.610642	3794.185278	23.017869
102.024258	3813.020550	23.022887
102.102519	3822.988579	23.027904
102.225656	3825.936205	23.032922
102.142236	3828.228111	23.037939
102.489471	3820.661596	23.042957
102.160449	3832.921812	23.047975
102.554052	3840.438473	23.052992
102.487078	3844.959336	23.058010
102.514404	3862.321200	23.063027
102.735528	3852.268295	23.068045
102.763971	3862.698663	23.073063
102.584654	3860.147989	23.078080
102.746921	3876.002088	23.083098
102.860385	3876.413537	23.088115
103.258722	3886.101041	23.093133
103.504297	3894.827704	23.098151
103.331007	3893.993133	23.103168
103.865035	3902.598855	23.108186
103.468515	3901.357369	23.113203
103.785914	3904.041003	23.118221
103.996902	3921.415181	23.123239
104.173449	3928.460870	23.128256
104.068738	3931.807191	23.133274
104.526117	3929.955313	23.138291
104.483359	3922.339384	23.143309
104.571125	3943.296410	23.148327
104.645856	3944.099005	23.153344
105.279386	3953.658163	23.158362
104.847873	3958.236166	23.163379
105.095168	3955.628111	23.168397
105.044691	3952.561690	23.173415
104.726271	3955.243942	23.178432
105.624282	3961.176047	23.183450
105.532652	3966.540394	23.188467
105.712504	3970.501818	23.193485
105.483723	3985.634501	23.198503
105.505487	3983.162779	23.203520
105.895111	3966.840129	23.208538
105.659072	3983.141800	23.213555
105.878247	3989.164485	23.218573
105.989404	4001.772491	23.223591
106.030717	4012.832203	23.228608
106.256447	4002.222973	23.233626
106.617188	4027.227979	23.238643
106.612829	4036.116965	23.243661
106.560295	4036.948972	23.248679
106.435349	4028.345305	23.253696
107.076435	4023.125198	23.258714
106.675564	4031.637568	23.263731
107.107139	4047.032983	23.268749
106.893480	4055.724354	23.273767
106.949300	4047.164954	23.278784
107.331997	4052.922158	23.283802
107.265011	4068.140034	23.288819
107.741140	4070.117047	23.293837
107.648477	4072.423058	23.298855
107.434767	4073.848466	23.303872
107.688251	4082.034239	23.308890
107.698742	4093.676446	23.313907
108.220473	4092.205862	23.318925
108.130358	4087.706319	23.323943
108.190767	4104.132099	23.328960
108.485608	4110.954161	23.333978
108.475331	4114.809680	23.338995
108.855362	4109.999745	23.344013
108.885658	4119.609311	23.349031
108.871243	4118.077529	23.354048
109.019171	4115.327199	23.359066
109.010212	4123.487823	23.364083
109.332572	4128.010888	23.369101
109.555534	4134.689557	23.374119
109.532819	4137.265536	23.379136
109.649397	4141.170627	23.384154
109.157704	4143.854801	23.389171
109.475297	4141.046322	23.394189
110.033556	4155.137332	23.399207
110.167639	4169.512599	23.404224
110.101019	4161.471039	23.409242
109.972359	4161.143955	23.414259
110.318789	4166.853219	23.419277
110.231661	4165.878881	23.424295
110.099765	4176.615469	23.429312
110.544260	4187.536368	23.434330
110.333680	4193.585418	23.439347
110.719028	4196.189009	23.444365
111.214080	4211.902886	23.449383
111.041172	4209.862495	23.454400
111.245343	4206.724572	23.459418
111.084414	4213.927406	23.464435
110.993524	4216.312067	23.469453
111.325323	4228.655246	23.474471
111.116365	4245.016036	23.479488
111.749559	4234.898362	23.484506
111.152538	4258.841680	23.489523
111.686193	4256.068774	23.494541
112.172528	4266.695933	23.499559
112.170589	4276.294850	23.504576
112.509940	4279.196050	23.509594
112.509449	4284.618810	23.514611
112.415888	4290.529615	23.519629
112.606230	4292.848131	23.524647
112.653674	4300.618072	23.529664
112.853951	4299.933280	23.534682
112.964834	4312.670958	23.539699
112.845797	4323.948523	23.544717
113.367897	4323.689930	23.549735
113.093028	4327.318651	23.554752
113.302051	4328.466369	23.559770
113.619101	4343.520148	23.564787
113.649214	4351.254949	23.569805
113.661485	4351.865336	23.574823
114.022604	4352.443165	23.579840
113.895901	4354.176918	23.584858
113.648375	4353.827420	23.589875
113.892227	4364.107541	23.594893
114.160115	4363.573132	23.599911
114.165881	4373.991565	23.604928
114.717480	4381.145962	23.609946
114.778561	4389.399896	23.614963
114.742509	4393.881329	23.619981
115.008672	4403.526691	23.624999
114.905019	4399.941401	23.630016
115.336328	4400.426167	23.635034
115.625032	4423.069367	23.640051
115.715053	4421.164520	23.645069
115.646166	4430.250039	23.650087
115.224887	4431.395506	23.655104
115.514385	4421.915516	23.660122
116.057492	4433.465028	23.665139
115.699178	4435.617004	23.670157
115.720606	4451.541018	23.675175
115.874569	4451.359038	23.680192
116.377374	4444.228734	23.685210
116.214581	4453.120650	23.690227
116.463030	4463.715752	23.695245
116.990135	4466.918995	23.700263
116.830158	4473.275854	23.705280
117.028238	4458.740914	23.710298
116.967634	4470.902689	23.715315
116.779963	4460.370586	23.720333
116.511568	4471.324432	23.725351
116.952711	4484.177782	23.730368
117.119472	4479.325408	23.735386
117.074097	4497.008601	23.740403
117.432146	4510.361080	23.745421
117.860843	4514.160537	23.750439
117.925992	4517.694992	23.755456
118.245151	4508.582772	23.760474
117.851489	4522.273982	23.765491
118.059718	4530.359728	23.770509
118.332959	4538.564709	23.775527
118.268353	4541.541865	23.780544
118.664597	4532.528033	23.785562
118.173387	4557.793504	23.790579
118.519004	4564.838204	23.795597
118.605090	4569.313172	23.800615
118.914844	4581.574821	23.805632
118.936406	4589.225839	23.810650
119.205734	4593.833084	23.815667
119.088601	4593.074907	23.820685
119.661239	4612.201745	23.825703
119.760301	4621.153726	23.830720
119.857603	4618.250273	23.835738
119.805051	4622.207217	23.840755
119.611135	4623.837892	23.845773
119.540171	4636.541158	23.850791
119.811708	4655.096545	23.855808
120.271253	4660.734584	23.860826
120.382181	4670.508572	23.865843
120.502358	4677.159354	23.870861
120.837651	4672.406785	23.875879
120.704873	4674.536081	23.880896
120.977250	4684.688812	23.885914
121.491193	4685.523637	23.890931
121.330163	4693.550518	23.895949
121.530851	4693.560074	23.900967
121.417525	4691.374565	23.905984
121.810002	4697.382962	23.911002
122.101608	4706.983465	23.916019
122.008414	4719.731306	23.921037
122.570243	4721.313032	23.926055
122.125056	4714.725704	23.931072
122.447638	4715.969290	23.936090
122.648287	4711.146267	23.941107
122.520723	4711.920616	23.946125
122.798861	4712.265252	23.951143
122.741379	4718.287333	23.956160
122.984020	4732.295669	23.961178
122.992614	4738.765096	23.966195
123.004258	4739.028380	23.971213
122.983548	4735.884564	23.976231
123.079267	4752.059192	23.981248
123.319960	4755.869215	23.986266
123.267853	4766.195932	23.991283
123.021106	4765.650600	23.996301
123.271826	4777.593355	24.001319
123.144995	4796.864693	24.006336
123.392309	4800.247561	24.011354
124.037709	4808.400671	24.016371
123.886098	4828.761764	24.021389
124.490310	4832.814720	24.026407
124.444181	4849.974393	24.031424
124.740518	4847.557389	24.036442
125.018639	4848.476516	24.041459
124.686522	4847.843547	24.046477
124.909920	4846.107151	24.051495
125.168180	4842.761786	24.056512
125.277590	4850.878940	24.061530
125.213787	4856.943092	24.066547
125.345645	4858.494341	24.071565
125.784503	4856.635806	24.076583
125.631061	4865.602215	24.081600
125.872232	4879.247895	24.086618
125.840051	4893.280471	24.091635
125.883720	4895.047557	24.096653
126.134957	4887.814450	24.101671
126.258739	4915.341987	24.106688
125.890736	4914.515777	24.111706
126.490247	4918.376941	24.116723
126.065290	4928.964181	24.121741
126.440867	4933.772668	24.126759
126.426776	4934.365110	24.131776
126.562122	4963.428136	24.136794
127.043241	4977.945379	24.141811
127.210711	4980.450646	24.146829
127.521518	4993.943458	24.151847
127.497004	4998.514773	24.156864
127.942853	4994.000480	24.161882
128.063948	4995.941682	24.166899
127.832158	5012.126815	24.171917
128.299099	5016.677957	24.176935
128.350501	5017.395872	24.181952
128.297409	5017.729276	24.186970
128.492894	5016.413901	24.191987
128.770969	5043.488169	24.197005
129.021617	5037.334634	24.202023
128.854193	5046.072894	24.207040
128.966662	5052.560881	24.212058
129.184978	5058.543023	24.217075
129.060417	5077.325037	24.222093
129.325932	5071.225980	24.227111
129.450765	5075.941214	24.232128
129.342871	5081.996565	24.237146
129.966881	5092.078653	24.242163
129.828348	5096.951945	24.247181
130.075468	5092.945403	24.252199
130.177543	5106.770873	24.257216
130.460449	5117.995427	24.262234
130.680927	5126.167904	24.267251
130.543680	5119.926754	24.272269
130.538438	5124.387758	24.277287
130.707219	5141.678177	24.282304
131.037089	5147.273553	24.287322
131.370931	5143.004045	24.292339
131.400628	5155.849731	24.297357
131.355664	5154.019617	24.302375
131.069386	5159.913547	24.307392
131.656558	5168.306373	24.312410
131.595425	5174.471222	24.317427
131.504554	5177.439971	24.322445
132.183831	5184.199054	24.327463
131.940351	5187.987168	24.332480
131.899336	5206.980344	24.337498
132.259343	5211.775562	24.342515
132.314264	5224.996133	24.347533
132.658025	5217.227566	24.352551
132.581123	5246.816723	24.357568
132.769715	5253.103460	24.362586
133.018219	5247.512063	24.367603
133.332995	5253.621203	24.372621
133.379483	5252.849990	24.377639
133.412762	5265.152260	24.382656
133.557759	5271.720457	24.387674
133.996770	5266.070799	24.392691
133.794930	5277.649175	24.397709
133.962963	5267.079815	24.402727
134.176182	5282.838776	24.407744
134.298474	5293.820292	24.412762
134.895850	5289.938759	24.417779
134.260516	5293.415808	24.422797
134.808278	5290.533217	24.427815
134.841254	5294.792567	24.432832
134.747051	5313.712115	24.437850
135.259731	5315.759302	24.442867
134.757353	5329.215619	24.447885
135.224850	5328.526805	24.452903
135.426985	5345.209282	24.457920
135.302181	5348.880983	24.462938
135.477297	5349.560590	24.467955
135.322940	5365.680243	24.472973
135.900325	5367.300627	24.477991
135.968760	5372.394096	24.483008
135.966566	5387.842826	24.488026
136.337040	5390.938198	24.493043
136.454826	5408.157944	24.498061
136.703864	5414.959265	24.503079
136.604567	5417.370652	24.508096
136.444843	5428.207035	24.513114
136.941822	5428.034440	24.518131
136.957533	5457.748320	24.523149
137.079057	5447.527058	24.528167
137.450904	5456.209437	24.533184
137.354407	5475.656668	24.538202
137.767104	5478.234067	24.543219
137.685064	5491.081711	24.548237
137.765140	5506.527122	24.553255
137.717912	5505.805303	24.558272
137.878319	5518.397176	24.563290
138.602966	5530.345093	24.568307
138.352118	5537.215305	24.573325
138.586925	5537.677230	24.578343
138.996545	5552.073556	24.583360
138.925833	5551.446957	24.588378
139.271105	5556.484479	24.593395
139.319122	5576.149080	24.598413
139.623110	5585.918567	24.603431
140.152130	5591.296639	24.608448
139.673658	5592.362748	24.613466
139.978612	5590.484083	24.618483
139.736743	5594.874948	24.623501
139.840807	5599.394702	24.628519
140.275355	5609.001698	24.633536
140.509328	5612.522544	24.638554
140.483426	5629.581925	24.643571
140.964075	5639.667838	24.648589
140.728002	5638.656779	24.653607
141.066006	5629.941945	24.658624
140.983168	5654.526248	24.663642
141.371258	5661.810942	24.668659
141.460640	5662.810188	24.673677
141.442510	5659.735254	24.678695
141.790736	5669.551519	24.683712
141.701148	5675.815694	24.688730
141.751228	5681.852808	24.693747
141.559292	5695.494350	24.698765
142.260752	5703.127705	24.703783
142.391011	5701.175385	24.708800
142.562350	5709.529440	24.713818
142.606140	5712.451925	24.718835
142.361754	5731.051357	24.723853
142.516317	5736.866937	24.728871
142.806021	5740.192833	24.733888
142.716886	5755.374551	24.738906
142.923697	5761.440800	24.743923
142.966173	5778.202350	24.748941
143.495831	5787.876614	24.753959
143.877049	5802.615352	24.758976
144.094589	5801.640544	24.763994
144.224901	5813.252451	24.769011
143.943115	5822.615081	24.774029
143.912673	5815.119540	24.779047
144.513193	5829.356754	24.784064
144.491676	5851.418997	24.789082
145.124907	5848.930144	24.794099
145.162795	5846.146288	24.799117
145.046578	5849.608402	24.804135
145.372566	5866.862253	24.809152
145.302966	5873.830463	24.814170
145.709502	5866.023378	24.819187
145.516097	5875.867788	24.824205
145.749999	5894.922779	24.829223
146.113453	5894.906839	24.834240
145.953102	5892.671731	24.839258
146.036665	5904.246827	24.844275
146.011821	5920.791772	24.849293
146.491548	5921.218493	24.854311
146.729806	5925.155413	24.859328
146.744415	5947.575132	24.864346
147.255820	5953.413794	24.869363
147.303386	5952.844412	24.874381
147.287298	5958.708895	24.879399
147.406264	5966.108477	24.884416
147.529170	5976.518944	24.889434
147.746592	5973.227123	24.894451
148.177022	5984.485921	24.899469
148.156948	5995.120828	24.904487
148.139446	5995.271899	24.909504
148.100933	6002.206877	24.914522
148.220780	6001.225267	24.919539
148.507010	6018.779065	24.924557
148.666690	6025.263159	24.929575
148.757636	6022.928688	24.934592
149.253687	6044.537586	24.939610
149.276871	6043.400655	24.944627
149.093606	6052.179757	24.949645
149.150427	6070.044178	24.954663
149.558403	6089.700290	24.959680
149.618957	6087.926156	24.964698
149.763060	6088.408619	24.969715
150.065378	6105.609583	24.974733
149.887859	6109.728480	24.979751
150.715185	6111.391853	24.984768
150.545037	6119.988999	24.989786
150.793117	6125.221840	24.994803
151.049169	6126.043477	24.999821
151.146539	6141.616142	25.004839
151.470535	6149.207806	25.009856
151.551139	6155.388661	25.014874
151.772012	6157.162832	25.019891
151.364570	6154.069888	25.024909
151.337337	6162.789874	25.029927
152.029242	6169.212736	25.034944
151.958701	6174.426060	25.039962
152.274075	6192.433186	25.044979
152.572357	6196.572263	25.049997
152.489558	6210.070820	25.055015
152.556771	6198.399230	25.060032
152.295175	6211.136612	25.065050
152.616828	6215.732917	25.070067
152.422554	6230.505339	25.075085
152.858776	6247.073049	25.080103
152.957138	6253.188019	25.085120
153.525368	6264.153921	25.090138
153.737597	6285.996975	25.095155
153.956281	6287.029664	25.100173
154.089024	6291.870244	25.105191
154.150290	6283.337353	25.110208
154.243423	6311.872489	25.115226
154.646549	6308.362110	25.120243
154.407856	6310.527127	25.125261
154.536254	6318.506219	25.130279
155.112925	6334.594274	25.135296
154.926750	6339.999383	25.140314
155.437457	6347.707090	25.145331
155.225269	6347.901291	25.150349
155.102940	6364.215680	25.155367
155.649045	6365.411739	25.160384
155.435945	6391.775763	25.165402
155.899635	6395.494374	25.170419
156.242738	6390.089845	25.175437
156.124771	6416.259063	25.180455
156.638826	6413.861413	25.185472
156.668734	6422.556787	25.190490
156.597512	6431.479512	25.195507
157.168363	6438.290779	25.200525
156.818460	6451.225255	25.205543
157.060891	6464.783534	25.210560
157.156443	6471.612453	25.215578
157.446733	6472.103593	25.220595
157.676066	6480.890867	25.225613
158.068659	6501.878842	25.230631
158.060603	6496.163107	25.235648
157.821328	6506.103430	25.240666
157.901383	6514.027046	25.245683
158.259016	6517.585517	25.250701
158.782711	6538.205747	25.255719
158.917614	6548.772500	25.260736
158.987550	6553.869220	25.265754
159.183739	6568.296629	25.270771
159.219442	6574.159508	25.275789
159.437306	6588.163681	25.280807
159.350923	6584.051223	25.285824
159.687049	6603.933807	25.290842
159.798010	6602.158041	25.295859
160.268687	6620.756837	25.300877
160.408046	6632.664589	25.305895
160.588232	6623.999265	25.310912
160.754957	6633.285726	25.315930
161.030456	6648.420529	25.320947
161.369415	6644.916982	25.325965
160.914586	6655.396247	25.330983
161.248566	6656.511913	25.336000
161.667182	6672.025230	25.341018
161.928852	6679.582684	25.346035
161.766517	6679.153496	25.351053
161.572945	6689.086758	25.356071
161.608548	6686.820853	25.361088
161.910593	6693.500702	25.366106
162.019037	6719.615942	25.371123
162.422220	6732.682024	25.376141
162.417616	6742.914022	25.381159
162.504546	6750.975563	25.386176
162.812463	6763.428381	25.391194
163.235278	6763.718828	25.396211
163.265991	6781.698523	25.401229
163.326278	6796.059010	25.406247
163.582898	6791.081460	25.411264
163.666069	6806.233896	25.416282
163.660163	6814.158480	25.421299
164.058535	6815.283009	25.426317
164.283308	6838.974672	25.431335
164.436840	6835.784257	25.436352
164.772343	6840.059708	25.441370
164.661630	6847.012630	25.446387
164.497710	6860.641177	25.451405
164.891934	6871.773607	25.456423
165.136850	6879.744160	25.461440
165.441825	6887.411720	25.466458
165.710121	6899.880308	25.471475
165.852667	6897.092525	25.476493
165.739344	6916.098800	25.481511
165.993828	6916.466131	25.486528
166.202559	6929.105071	25.491546
166.326589	6943.061078	25.496563
166.959504	6941.778059	25.501581
167.121716	6949.638482	25.506599
166.985722	6950.553146	25.511616
166.945151	6963.733109	25.516634
167.203525	6966.148645	25.521651
167.352139	6971.091096	25.526669
167.422191	6996.893899	25.531687
167.822285	7005.910380	25.536704
167.856820	7005.355635	25.541722
167.563114	7017.984956	25.546739
168.384523	7023.311336	25.551757
168.597397	7049.240211	25.556775
168.497535	7050.079768	25.561792
168.694536	7054.146515	25.566810
169.078219	7069.293128	25.571827
169.069424	7073.597318	25.576845
169.394391	7082.729785	25.581863
169.289330	7083.926887	25.586880
169.758453	7101.838212	25.591898
169.991422	7116.200309	25.596915
169.993789	7121.033121	25.601933
170.162304	7140.213300	25.606951
170.281241	7139.585347	25.611968
170.422686	7142.423310	25.616986
170.433384	7162.205950	25.622003
170.954255	7162.272687	25.627021
170.966383	7176.846215	25.632039
170.989354	7186.392247	25.637056
171.136232	7193.102902	25.642074
171.619262	7205.635922	25.647091
172.151451	7208.276932	25.652109
171.725813	7220.554544	25.657127
172.128934	7232.932785	25.662144
172.525963	7243.616719	25.667162
172.300466	7253.302733	25.672180
172.519267	7242.825306	25.677197
172.588885	7263.946832	25.682215
172.793541	7268.091351	25.687232
173.292560	7274.071285	25.692250
173.231117	7292.470004	25.697268
173.197872	7302.530012	25.702285
173.312527	7308.974261	25.707303
173.886066	7309.660979	25.712320
173.867677	7325.890484	25.717338
173.757415	7331.078788	25.722356
174.120143	7339.671944	25.727373
174.379030	7353.897575	25.732391
174.328011	7354.012867	25.737408
174.613574	7367.429308	25.742426
174.549407	7374.188877	25.747444
174.730630	7381.418273	25.752461
174.859234	7395.847450	25.757479
175.008076	7397.996078	25.762496
175.492838	7413.493347	25.767514
175.759613	7430.956837	25.772532
175.887579	7433.421278	25.777549
175.952316	7450.853300	25.782567
176.057468	7456.869743	25.787584
176.349779	7470.679823	25.792602
176.352397	7486.546285	25.797620
176.810927	7479.330199	25.802637
177.176762	7512.051653	25.807655
177.191806	7509.687845	25.812672
177.455009	7501.833073	25.817690
177.286763	7533.062907	25.822708
177.323515	7537.476878	25.827725
177.574870	7545.415143	25.832743
177.462295	7558.641539	25.837760
178.192288	7568.967273	25.842778
178.108886	7580.446461	25.847796
178.440549	7596.937063	25.852813
178.498107	7611.428051	25.857831
178.707928	7618.709886	25.862848
179.320844	7641.063195	25.867866
179.406470	7649.826187	25.872884
179.597480	7644.539831	25.877901
179.574062	7665.701648	25.882919
179.894578	7669.247219	25.887936
180.158272	7682.206395	25.892954
180.133380	7698.411991	25.897972
180.743151	7690.540729	25.902989
180.691477	7705.418272	25.908007
180.706096	7725.690238	25.913024
181.160661	7724.289888	25.918042
180.996530	7738.099064	25.923060
181.545548	7747.291472	25.928077
181.682935	7752.283247	25.933095
181.599250	7764.113022	25.938112
182.147276	7768.030225	25.943130
182.219559	7778.064489	25.948148
182.412128	7781.626969	25.953165
182.667693	7798.887359	25.958183
182.908816	7812.140608	25.963200
183.285891	7805.533834	25.968218
182.961710	7807.084169	25.973236
183.049525	7830.482863	25.978253
183.459392	7824.079309	25.983271
183.383376	7837.230722	25.988288
183.829550	7852.197713	25.993306
183.935357	7863.536938	25.998324
183.974488	7872.591453	26.003341
184.232979	7880.803407	26.008359
184.338087	7890.763135	26.013376
184.836372	7903.613103	26.018394
184.835479	7917.744115	26.023412
184.998229	7914.520500	26.028429
185.313492	7920.261086	26.033447
185.266486	7944.596587	26.038464
185.722607	7942.883431	26.043482
185.421638	7961.866509	26.048500
185.579332	7965.125098	26.053517
185.888625	7978.323589	26.058535
185.947937	7991.659119	26.063552
186.166496	8003.271216	26.068570
186.368482	8021.755674	26.073588
186.207420	8028.136028	26.078605
186.864095	8049.958907	26.083623
186.760686	8054.025583	26.088640
187.381057	8068.144623	26.093658
187.239279	8086.578817	26.098676
187.600222	8093.243636	26.103693
187.747809	8098.776924	26.108711
187.511171	8118.533037	26.113728
188.220118	8123.823693	26.118746
188.419441	8137.386803	26.123764
188.861871	8149.614278	26.128781
188.811806	8165.328565	26.133799
188.982785	8163.596918	26.138816
189.346709	8176.695437	26.143834
189.698082	8196.526842	26.148852
189.802440	8202.865676	26.153869
189.818866	8204.788890	26.158887
189.573489	8226.424956	26.163904
189.774168	8231.084922	26.168922
190.041567	8241.360381	26.173940
190.158379	8250.134558	26.178957
190.660521	8268.117618	26.183975
190.719445	8275.186571	26.188992
191.280772	8286.947203	26.194010
191.292822	8304.669266	26.199028
191.583681	8309.043613	26.204045
191.780335	8328.593159	26.209063
191.852102	8330.908670	26.214080
191.930049	8337.096989	26.219098
191.962154	8354.014051	26.224116
192.182696	8370.219671	26.229133
192.806582	8378.412490	26.234151
192.704525	8386.605381	26.239168
193.367041	8400.635989	26.244186
193.270054	8420.263205	26.249204
193.451858	8429.358784	26.254221
193.855785	8442.571195	26.259239
193.701784	8445.070474	26.264256
194.043958	8448.499148	26.269274
194.375540	8468.412874	26.274292
194.312789	8475.532536	26.279309
194.809446	8490.410051	26.284327
194.990854	8500.942225	26.289344
194.816143	8509.399124	26.294362
194.981194	8519.321386	26.299380
194.945432	8536.116647	26.304397
195.372515	8549.805394	26.309415
195.631578	8560.963181	26.314432
195.867810	8579.332331	26.319450
196.126214	8588.179202	26.324468
196.262338	8604.477181	26.329485
196.902733	8595.060050	26.334503
196.894325	8618.241185	26.339520
196.692154	8622.231899	26.344538
196.900072	8639.557368	26.349556
197.036548	8652.802357	26.354573
197.596165	8671.225124	26.359591
197.407607	8688.786394	26.364608
197.801833	8693.864475	26.369626
198.239785	8711.034001	26.374644
198.086847	8719.089780	26.379661
198.746571	8729.986000	26.384679
198.995162	8742.443138	26.389696
199.377947	8744.561590	26.394714
199.441596	8751.371095	26.399732
199.415847	8775.483355	26.404749
199.582428	8776.158117	26.409767
199.601483	8785.427755	26.414784
200.010594	8794.494219	26.419802
199.975831	8796.261340	26.424820
200.211499	8792.486270	26.429837
200.337688	8813.067139	26.434855
200.405129	8827.244968	26.439872
201.068862	8836.120018	26.444890
201.028164	8859.369657	26.449908
200.982477	8862.903371	26.454925
201.604448	8868.151040	26.459943
201.545153	8889.502994	26.464960
201.686398	8894.497631	26.469978
201.889415	8909.033149	26.474996
201.915240	8921.638965	26.480013
202.602588	8931.359651	26.485031
202.145349	8947.529883	26.490048
202.945814	8965.785767	26.495066
203.044042	8974.146446	26.500084
203.484229	8991.786308	26.505101
203.677316	8997.988383	26.510119
203.744340	9010.654108	26.515136
203.993477	9025.450856	26.520154
204.006959	9032.836625	26.525172
203.852672	9043.368024	26.530189
204.480884	9056.018481	26.535207
204.532940	9081.104006	26.540224
204.821310	9083.234131	26.545242
204.997607	9099.949322	26.550260
205.149059	9119.355236	26.555277
205.555546	9132.201499	26.560295
205.708177	9141.560893	26.565312
206.106642	9145.031396	26.570330
206.529099	9159.905288	26.575348
206.148459	9174.103062	26.580365
206.888681	9177.441100	26.585383
206.876569	9191.369618	26.590400
207.048487	9201.891049	26.595418
207.303524	9219.424372	26.600436
207.302538	9223.702580	26.605453
207.822696	9232.025692	26.610471
208.251366	9251.359900	26.615488
208.206738	9250.849063	26.620506
208.180516	9259.671384	26.625524
207.903994	9281.600868	26.630541
208.426799	9292.108426	26.635559
208.590521	9311.976738	26.640576
209.250832	9326.046284	26.645594
209.262540	9342.108662	26.650612
209.296184	9356.595289	26.655629
209.827603	9365.052461	26.660647
209.758442	9379.640458	26.665664
209.903032	9390.349399	26.670682
210.278819	9400.526433	26.675700
210.211775	9414.940475	26.680717
210.356170	9430.312796	26.685735
210.808241	9444.512931	26.690752
210.767598	9461.455028	26.695770
211.026426	9483.165119	26.700788
211.379501	9500.746495	26.705805
212.018406	9516.631835	26.710823
212.083473	9519.330580	26.715840
212.025801	9528.031662	26.720858
212.235197	9550.554691	26.725876
212.522753	9569.504043	26.730893
212.724037	9578.770787	26.735911
212.950876	9586.278061	26.740928
213.175094	9595.610683	26.745946
213.593564	9615.073161	26.750964
213.718915	9639.699615	26.755981
213.988862	9628.073036	26.760999
214.117618	9631.361713	26.766016
214.643025	9652.083039	26.771034
214.865568	9661.779050	26.776052
214.844864	9674.730501	26.781069
214.997576	9684.371159	26.786087
215.572799	9693.910902	26.791104
215.267724	9698.366308	26.796122
215.672297	9714.869480	26.801140
215.663348	9716.061165	26.806157
215.941338	9729.799401	26.811175
216.035664	9746.619578	26.816192
216.281674	9761.297423	26.821210
216.627476	9771.012070	26.826228
216.602846	9794.165638	26.831245
216.872950	9801.034749	26.836263
217.255680	9817.863485	26.841280
216.724588	9834.046051	26.846298
217.530384	9847.749050	26.851316
217.955454	9872.619338	26.856333
218.123802	9883.037520	26.861351
218.164690	9893.936653	26.866368
218.407148	9917.219031	26.871386
219.132040	9920.553294	26.876404
219.121677	9938.671942	26.881421
219.326591	9944.967202	26.886439
219.597901	9979.340192	26.891456
219.636825	9982.845077	26.896474
220.135195	9994.862938	26.901492
220.327262	10012.327938	26.906509
220.908722	10012.202080	26.911527
220.698750	10028.110333	26.916544
220.811867	10037.905775	26.921562
221.143386	10052.062113	26.926580
220.923199	10065.755501	26.931597
221.864533	10077.817689	26.936615
221.831791	10078.526883	26.941632
221.570175	10095.387349	26.946650
221.613525	10116.746730	26.951668
221.861683	10139.747483	26.956685
222.353434	10150.487727	26.961703
223.030561	10164.138497	26.966720
222.812332	10189.078410	26.971738
223.282861	10189.711925	26.976756
223.110075	10210.505362	26.981773
223.531279	10233.731716	26.986791
223.869468	10249.727943	26.991808
224.114057	10271.327515	26.996826
224.450480	10287.011464	27.001844
224.827784	10290.583380	27.006861
225.071067	10312.233724	27.011879
225.377992	10316.842840	27.016896
225.432747	10330.562815	27.021914
225.823896	10335.717610	27.026932
225.728715	10354.052025	27.031949
225.803717	10378.766278	27.036967
225.995920	10379.092925	27.041984
226.561611	10397.295435	27.047002
226.875854	10411.413705	27.052020
227.136052	10431.287042	27.057037
227.422283	10435.201630	27.062055
227.507915	10445.708864	27.067072
227.524354	10459.362313	27.072090
227.857874	10468.046756	27.077108
228.186123	10480.650454	27.082125
227.951393	10490.724807	27.087143
228.358398	10504.557073	27.092160
228.418962	10518.838307	27.097178
228.693444	10526.600568	27.102196
228.903867	10547.321716	27.107213
229.041615	10570.251886	27.112231
229.608480	10576.939023	27.117248
229.556976	10595.298406	27.122266
229.990079	10605.227153	27.127284
230.319107	10621.834531	27.132301
230.631186	10625.126240	27.137319
230.686106	10646.639132	27.142336
230.821351	10658.338565	27.147354
231.219666	10682.086894	27.152372
231.035109	10691.367274	27.157389
231.447076	10707.895429	27.162407
232.024986	10722.206286	27.167424
232.312946	10736.565733	27.172442
232.205642	10743.885848	27.177460
232.305055	10756.746608	27.182477
232.683018	10762.664552	27.187495
233.278060	10789.508148	27.192512
232.691435	10805.993899	27.197530
233.490840	10820.225928	27.202548
233.620306	10843.915538	27.207565
233.800860	10857.300438	27.212583
234.282343	10869.839347	27.217600
234.721131	10889.359968	27.222618
234.590011	10902.007496	27.227636
235.069165	10913.438500	27.232653
235.146847	10927.461603	27.237671
235.406749	10937.054541	27.242688
235.627466	10949.811177	27.247706
236.139528	10965.938658	27.252724
235.961530	10985.382336	27.257741
236.348049	10995.568036	27.262759
236.576397	11002.892506	27.267776
236.643905	11022.736664	27.272794
237.052727	11045.792302	27.277812
237.340153	11054.825257	27.282829
237.596593	11073.698915	27.287847
237.801506	11087.515909	27.292864
238.051475	11112.923650	27.297882
238.086614	11117.382930	27.302900
238.225992	11145.185699	27.307917
238.442533	11155.189713	27.312935
238.662113	11166.809943	27.317952
238.880489	11196.008698	27.322970
239.190764	11208.063125	27.327988
239.670827	11222.187608	27.333005
239.838348	11241.567950	27.338023
240.005193	11261.017886	27.343040
240.166137	11284.791535	27.348058
240.626240	11292.262955	27.353076
240.715679	11319.739099	27.358093
240.986548	11332.412356	27.363111
241.437009	11351.694809	27.368128
241.309785	11364.872519	27.373146
241.959886	11375.026608	27.378164
241.621677	11397.805002	27.383181
241.962215	11413.656607	27.388199
242.629816	11433.470344	27.393216
242.716218	11439.888878	27.398234
242.984067	11454.334125	27.403252
242.900808	11481.499692	27.408269
243.428767	11498.566120	27.413287
243.877968	11508.628606	27.418304
243.835693	11523.053020	27.423322
244.531746	11544.093902	27.428340
244.848432	11555.310769	27.433357
244.794833	11573.153581	27.438375
245.089253	11578.693322	27.443392
245.134089	11601.794033	27.448410
245.681747	11602.551300	27.453428
245.963575	11618.535425	27.458445
245.836936	11636.733924	27.463463
246.002726	11645.271519	27.468480
246.376985	11660.789652	27.473498
246.687308	11677.476682	27.478516
247.114519	11687.091161	27.483533
246.757327	11702.944952	27.488551
247.413946	11712.280364	27.493568
247.386973	11737.337624	27.498586
247.518369	11754.624293	27.503604
248.246760	11772.126911	27.508621
248.555031	11804.249183	27.513639
248.793880	11802.781293	27.518656
248.644595	11822.252913	27.523674
248.823842	11842.983535	27.528692
249.228516	11864.989315	27.533709
249.256004	11865.524940	27.538727
249.674208	11879.492252	27.543744
249.953841	11916.115782	27.548762
250.290998	11926.796011	27.553780
250.616707	11940.929428	27.558797
250.554781	11956.831909	27.563815
250.943320	11970.946033	27.568832
250.747989	12000.883442	27.573850
251.008048	12016.403971	27.578868
251.288616	12043.683871	27.583885
251.994135	12067.430040	27.588903
252.317368	12084.598543	27.593920
252.489431	12109.874580	27.598938
252.930060	12132.639216	27.603956
253.124201	12144.744016	27.608973
253.758120	12161.917602	27.613991
253.696653	12176.045535	27.619008
253.950825	12184.544268	27.624026
254.078975	12194.657416	27.629044
254.901055	12225.692592	27.634061
254.885630	12230.216896	27.639079
255.495151	12244.274504	27.644096
255.536524	12258.923211	27.649114
255.701691	12279.621784	27.654132
256.136136	12278.015852	27.659149
256.377794	12309.198930	27.664167
256.559547	12307.626266	27.669184
256.647347	12322.371956	27.674202
256.683737	12330.105950	27.679220
257.202590	12349.865015	27.684237
257.315712	12371.876009	27.689255
258.027607	12384.414576	27.694272
257.757391	12404.272044	27.699290
257.835557	12415.211011	27.704308
258.312571	12437.881898	27.709325
258.715698	12454.905596	27.714343
258.782558	12463.882206	27.719360
259.184879	12482.734428	27.724378
259.377033	12500.962765	27.729396
259.666885	12518.891612	27.734413
259.686530	12552.850857	27.739431
260.052899	12561.982696	27.744448
260.439370	12579.419633	27.749466
260.407490	12595.696884	27.754484
260.613399	12616.121028	27.759501
260.962187	12639.904856	27.764519
260.941386	12662.660313	27.769536
261.348253	12670.292202	27.774554
261.986239	12693.064493	27.779572
261.881000	12701.351345	27.784589
262.196212	12730.322576	27.789607
262.425224	12742.794923	27.794624
262.832770	12762.751855	27.799642
262.997085	12777.688017	27.804660
263.249389	12791.445156	27.809677
262.928261	12820.800417	27.814695
263.633215	12838.929802	27.819712
264.084074	12860.092674	27.824730
264.346216	12881.954603	27.829748
264.538825	12892.020133	27.834765
264.450036	12903.945532	27.839783
264.888067	12921.921023	27.844800
264.886125	12954.608585	27.849818
265.066957	12978.185466	27.854836
265.743050	13000.203738	27.859853
265.654156	13035.415589	27.864871
266.246925	13052.492225	27.869888
266.683426	13078.236556	27.874906
267.085611	13097.180992	27.879924
267.691629	13116.402992	27.884941
267.535990	13136.372753	27.889959
267.740947	13151.666004	27.894976
268.039454	13168.978317	27.899994
268.266496	13187.542907	27.905012
268.793960	13209.379442	27.910029
268.610043	13238.249637	27.915047
269.274905	13257.112032	27.920064
269.386259	13276.692741	27.925082
269.409705	13296.429350	27.930100
269.911799	13306.613991	27.935117
270.199867	13337.118850	27.940135
270.714428	13348.015259	27.945152
270.783135	13376.814512	27.950170
270.883216	13401.633016	27.955188
271.652672	13414.763268	27.960205
271.781060	13450.712396	27.965223
272.065284	13455.360584	27.970240
272.640501	13480.868991	27.975258
272.507560	13489.413163	27.980276
273.047668	13508.210086	27.985293
273.115518	13528.682106	27.990311
273.470380	13548.701807	27.995328
273.475662	13567.156240	28.000346
273.784503	13587.969532	28.005364
274.076431	13604.354823	28.010381
274.324658	13637.623340	28.015399
274.572110	13647.867003	28.020416
274.613847	13676.115126	28.025434
275.044836	13703.307540	28.030452
275.299718	13726.261096	28.035469
275.888117	13749.787722	28.040487
276.170319	13768.536880	28.045504
276.246710	13783.042326	28.050522
276.326991	13807.930781	28.055540
276.948990	13825.811994	28.060557
277.034701	13838.560155	28.065575
277.577071	13870.169245	28.070592
277.780846	13887.850756	28.075610
277.768328	13913.698142	28.080628
278.432184	13927.587436	28.085645
278.375008	13956.413603	28.090663
278.557581	13975.039617	28.095680
279.156838	13996.960555	28.100698
279.163817	14020.572281	28.105716
279.532481	14042.289381	28.110733
279.915294	14060.072487	28.115751
280.197310	14080.059946	28.120768
280.721008	14100.094836	28.125786
280.870994	14125.130690	28.130804
281.356360	14133.998320	28.135821
281.213647	14159.724320	28.140839
281.449062	14169.269055	28.145856
282.134672	14186.265853	28.150874
282.126887	14218.034339	28.155892
282.212209	14219.811579	28.160909
282.827150	14234.539342	28.165927
283.264257	14253.381563	28.170944
283.595517	14268.071679	28.175962
283.191822	14294.088234	28.180980
283.452985	14320.101735	28.185997
283.846282	14347.708373	28.191015
284.734733	14363.814546	28.196032
284.729458	14374.748765	28.201050
284.362423	14397.323676	28.206068
284.979760	14420.309720	28.211085
285.541809	14445.736218	28.216103
285.844748	14480.744089	28.221120
286.037777	14496.640340	28.226138
286.017314	14519.356910	28.231156
286.546652	14542.890614	28.236173
286.517383	14572.749215	28.241191
287.220905	14595.848297	28.246208
287.631345	14613.333883	28.251226
287.821202	14639.210556	28.256244
288.184757	14660.922846	28.261261
288.437030	14683.360025	28.266279
288.567238	14714.198165	28.271296
289.190295	14736.030958	28.276314
289.137700	14754.621935	28.281332
289.451106	14767.000281	28.286349
289.701944	14791.455896	28.291367
289.889009	14818.647058	28.296384
290.046326	14838.654848	28.301402
290.583689	14857.917795	28.306420
291.115599	14880.608272	28.311437
290.993277	14905.719390	28.316455
291.719820	14934.316886	28.321472
292.035962	14956.832812	28.326490
291.997865	14984.896410	28.331508
292.504534	15006.785644	28.336525
292.460511	15030.030779	28.341543
292.583878	15050.833667	28.346560
293.092368	15078.060120	28.351578
293.478174	15109.149417	28.356596
293.958933	15130.076428	28.361613
294.225179	15160.489722	28.366631
294.330864	15180.540699	28.371648
294.904452	15195.556770	28.376666
294.886341	15227.887565	28.381684
295.240206	15245.925816	28.386701
295.759968	15278.835677	28.391719
295.738087	15297.975068	28.396736
296.357033	15316.537194	28.401754
296.445347	15345.472154	28.406772
297.010686	15368.878065	28.411789
297.535250	15397.962690	28.416807
297.767033	15413.319881	28.421824
297.940098	15435.827201	28.426842
298.294052	15452.845502	28.431860
298.628586	15464.674605	28.436877
298.685620	15491.839719	28.441895
298.997481	15522.941272	28.446912
299.252707	15527.108131	28.451930
299.630458	15568.135502	28.456948
299.984913	15575.609384	28.461965
300.296535	15603.132724	28.466983
300.452997	15620.166319	28.472000
300.751950	15633.277067	28.477018
300.960064	15654.301052	28.482036
301.404434	15680.079256	28.487053
301.727467	15696.755200	28.492071
301.638362	15733.216449	28.497088
302.143410	15741.516403	28.502106
302.134482	15768.733299	28.507124
302.811399	15794.936350	28.512141
302.866080	15813.985303	28.517159
302.871888	15845.286923	28.522176
303.344084	15869.497630	28.527194
303.623874	15892.942596	28.532212
303.908207	15920.341172	28.537229
304.378787	15958.048011	28.542247
304.587498	15989.643395	28.547264
304.947210	16010.558747	28.552282
305.147940	16033.109810	28.557300
305.715085	16061.936101	28.562317
306.157501	16082.026866	28.567335
306.006718	16113.811420	28.572352
306.813432	16136.722491	28.577370
307.212597	16173.000701	28.582388
307.344242	16194.580505	28.587405
307.738959	16226.933591	28.592423
307.877039	16246.333128	28.597440
308.339221	16257.466821	28.602458
308.427082	16290.739810	28.607476
308.517635	16315.851009	28.612493
309.260218	16346.709552	28.617511
309.442804	16365.802186	28.622528
310.123242	16387.795276	28.627546
310.079793	16415.871279	28.632564
310.198308	16442.983888	28.637581
311.294762	16466.980698	28.642599
311.012082	16490.884044	28.647616
311.696289	16510.267785	28.652634
311.854214	16539.143103	28.657652
311.971975	16566.057018	28.662669
312.513456	16584.695680	28.667687
312.551485	16616.963163	28.672704
312.839555	16648.243981	28.677722
312.977944	16670.240185	28.682740
313.458850	16692.473342	28.687757
313.984443	16726.436556	28.692775
313.915317	16754.138052	28.697792
314.224197	16779.288300	28.702810
314.914688	16807.502586	28.707828
315.363940	16832.776208	28.712845
315.432877	16851.536529	28.717863
315.626519	16880.378336	28.722880
316.233686	16909.382824	28.727898
316.506881	16937.722681	28.732916
317.035936	16962.642849	28.737933
317.066045	16990.019600	28.742951
317.627937	17017.028819	28.747968
317.696055	17036.787552	28.752986
317.835372	17063.989373	28.758004
318.122111	17096.881998	28.763021
318.813144	17119.768144	28.768039
319.016828	17150.121739	28.773056
319.412117	17168.771233	28.778074
319.647184	17197.281690	28.783092
320.123242	17221.976760	28.788109
320.704231	17240.950998	28.793127
320.490759	17257.655483	28.798144
320.430438	17286.768257	28.803162
320.982268	17310.194446	28.808180
321.180504	17344.611171	28.813197
321.755386	17361.697633	28.818215
321.968088	17396.680735	28.823232
322.339054	17409.907760	28.828250
322.419208	17448.777877	28.833268
322.953187	17484.620498	28.838285
322.927657	17498.869918	28.843303
323.583620	17535.072561	28.848320
323.982718	17563.223047	28.853338
324.210108	17585.297951	28.858356
324.500080	17614.950173	28.863373
324.984040	17636.909138	28.868391
325.643725	17665.467483	28.873408
325.700204	17691.839799	28.878426
325.915767	17724.959431	28.883444
325.917232	17749.988529	28.888461
326.291311	17767.694320	28.893479
326.447787	17800.564325	28.898496
327.337700	17829.977599	28.903514
327.402996	17866.077548	28.908532
327.792068	17891.639949	28.913549
327.713121	17921.659982	28.918567
328.283209	17951.155126	28.923584
328.774390	17987.548681	28.928602
328.983444	18015.097849	28.933620
329.261453	18049.667584	28.938637
329.777881	18072.127354	28.943655
330.080301	18107.900005	28.948672
330.499659	18141.733887	28.953690
331.019876	18166.669629	28.958708
331.178810	18196.558062	28.963725
331.808112	18222.866639	28.968743
331.949482	18260.307352	28.973760
332.350395	18279.096022	28.978778
332.871614	18302.679830	28.983796
333.118949	18329.989699	28.988813
333.537511	18351.321647	28.993831
333.976985	18385.342330	28.998848
334.213620	18398.572121	29.003866
334.417846	18431.726322	29.008884
334.587818	18456.218211	29.013901
335.301885	18473.991425	29.018919
335.275639	18512.545506	29.023936
335.615658	18534.919729	29.028954
335.914479	18569.145977	29.033972
336.233076	18602.086707	29.038989
336.785440	18623.473806	29.044007
336.756992	18654.459976	29.049024
336.946138	18684.218073	29.054042
337.417076	18712.832799	29.059060
337.858540	18756.361919	29.064077
338.292016	18772.043982	29.069095
338.443708	18802.534660	29.074112
338.985124	18838.561833	29.079130
339.320067	18865.542845	29.084148
339.705436	18909.036870	29.089165
340.162085	18923.489784	29.094183
340.198163	18946.209024	29.099200
340.882210	18982.163578	29.104218
341.011910	19010.895372	29.109236
341.193726	19033.730876	29.114253
341.770591	19069.639204	29.119271
342.345282	19098.781575	29.124288
342.651516	19128.465148	29.129306
342.991468	19158.484647	29.134324
343.416417	19181.838208	29.139341
343.446168	19194.551296	29.144359
343.741594	19228.539157	29.149376
344.165576	19253.617725	29.154394
344.472457	19271.752393	29.159412
344.645342	19311.818416	29.164429
344.823955	19333.372246	29.169447
345.270419	19362.446647	29.174464
345.655178	19389.231044	29.179482
346.007562	19407.864142	29.184500
346.295381	19450.875541	29.189517
346.645340	19472.010974	29.194535
347.292563	19499.784231	29.199552
347.463836	19530.892137	29.204570
348.086494	19559.913961	29.209588
348.165527	19590.151897	29.214605
348.660204	19616.243367	29.219623
348.972130	19647.177795	29.224640
349.245070	19667.579982	29.229658
349.301749	19705.327361	29.234676
349.343129	19730.915052	29.239693
349.972602	19761.711468	29.244711
350.234566	19799.363692	29.249728
350.442302	19834.516222	29.254746
351.391174	19865.970391	29.259764
351.510448	19907.871948	29.264781
351.639141	19930.723139	29.269799
352.000586	19970.381891	29.274816
351.936692	20003.846120	29.279834
352.546438	20039.909033	29.284852
353.272361	20079.435096	29.289869
353.551551	20116.851461	29.294887
354.297731	20142.809466	29.299904
354.590662	20176.906774	29.304922
354.961441	20210.739220	29.309940
355.327000	20240.686870	29.314957
355.604262	20271.065396	29.319975
356.021252	20301.845400	29.324992
356.358024	20334.426068	29.330010
356.792887	20359.182122	29.335028
357.104755	20398.173457	29.340045
357.654903	20413.857520	29.345063
357.776363	20446.693238	29.350080
358.208318	20488.389099	29.355098
358.603771	20510.516810	29.360116
359.242955	20550.177456	29.365133
359.394338	20572.558289	29.370151
359.572144	20601.101651	29.375168
360.034943	20634.996234	29.380186
360.524715	20649.154598	29.385204
360.718581	20700.100283	29.390221
361.230310	20727.220448	29.395239
361.242429	20755.960582	29.400256
361.575895	20789.401815	29.405274
362.142250	20823.798607	29.410292
362.471395	20850.062972	29.415309
362.959319	20877.123890	29.420327
363.219367	20907.316545	29.425344
363.638079	20948.800632	29.430362
364.077357	20971.389559	29.435380
364.234771	21008.226449	29.440397
364.812142	21032.367099	29.445415
365.272280	21070.970075	29.450432
365.131715	21106.179438	29.455450
365.943618	21125.007565	29.460468
365.972188	21162.541000	29.465485
366.492097	21193.002993	29.470503
366.978251	21219.135843	29.475520
367.058726	21263.826497	29.480538
367.617349	21285.285035	29.485556
367.733108	21312.859780	29.490573
368.204065	21342.881058	29.495591
368.747982	21365.536188	29.500608
369.056995	21407.499677	29.505626
369.060771	21429.196927	29.510644
369.616517	21463.691278	29.515661
370.290712	21491.779063	29.520679
370.773939	21518.228696	29.525696
371.055833	21547.300522	29.530714
371.122049	21577.752035	29.535732
371.433389	21613.573924	29.540749
371.612823	21651.501684	29.545767
371.849367	21674.205315	29.550784
372.219055	21716.065176	29.555802
372.483902	21754.219862	29.560820
372.790396	21792.684032	29.565837
373.270927	21820.903719	29.570855
373.350821	21857.141424	29.575872
373.703197	21904.767036	29.580890
374.470740	21943.115049	29.585908
374.955903	21987.737631	29.590925
375.105146	22027.042003	29.595943
375.504151	22060.740512	29.600960
375.943574	22116.453636	29.605978
376.389545	22141.753607	29.610996
376.593646	22179.962860	29.616013
377.009579	22228.779866	29.621031
377.807200	22250.619060	29.626048
378.087690	22295.994740	29.631066
378.828225	22329.595978	29.636084
378.952903	22376.127319	29.641101
379.327928	22402.424476	29.646119
379.839617	22437.426617	29.651136
380.048790	22477.904124	29.656154
380.485251	22504.709941	29.661172
380.947777	22554.228166	29.666189
381.201069	22592.853876	29.671207
381.856115	22620.838844	29.676224
381.852306	22661.128923	29.681242
382.563492	22694.015018	29.686260
383.187427	22728.210222	29.691277
383.415407	22770.637938	29.696295
383.857881	22786.505053	29.701312
383.830892	22833.168643	29.706330
384.589215	22860.107777	29.711348
384.805586	22905.874034	29.716365
385.139949	22934.402560	29.721383
385.482201	22971.744947	29.726400
385.772925	23000.311998	29.731418
386.428873	23051.115526	29.736436
386.645953	23075.795359	29.741453
387.150407	23110.983074	29.746471
387.414658	23142.037875	29.751488
387.683325	23186.071472	29.756506
388.468126	23217.607254	29.761524
388.742083	23260.686001	29.766541
388.671934	23302.365338	29.771559
389.537645	23330.969182	29.776576
389.638499	23375.983677	29.781594
389.914343	23418.500064	29.786612
390.512289	23454.899664	29.791629
390.778525	23494.182291	29.796647
391.576728	23520.111320	29.801664
391.705067	23561.267209	29.806682
392.119617	23593.247054	29.811700
392.564041	23629.633105	29.816717
392.209520	23676.590102	29.821735
392.876977	23715.330055	29.826752
393.561340	23758.111779	29.831770
394.074644	23784.193206	29.836788
394.508008	23826.243437	29.841805
394.374602	23852.015496	29.846823
395.013648	23891.139400	29.851840
395.373583	23940.626587	29.856858
396.200510	23972.447656	29.861876
396.580552	23998.404892	29.866893
396.658049	24038.179466	29.871911
397.286206	24059.965047	29.876928
397.650341	24107.050623	29.881946
397.732365	24135.633032	29.886964
398.273503	24171.935408	29.891981
398.445641	24215.316536	29.896999
399.103279	24254.495115	29.902016
399.269346	24294.837714	29.907034
399.391142	24334.334200	29.912052
400.407577	24369.962138	29.917069
400.800613	24415.287096	29.922087
401.162408	24451.668627	29.927104
401.257960	24494.044914	29.932122
401.817145	24535.975817	29.937140
402.264065	24562.498387	29.942157
402.518354	24614.165069	29.947175
402.807562	24659.506842	29.952192
403.435513	24705.269628	29.957210
403.830738	24737.033143	29.962228
404.225296	24766.926211	29.967245
404.693251	24835.009933	29.972263
405.318246	24863.173389	29.977280
405.314427	24909.263104	29.982298
405.555406	24951.630216	29.987316
406.256796	24988.471421	29.992333
406.563880	25035.068857	29.997351
407.559266	25069.247810	30.002368
407.659356	25120.093106	30.007386
407.892094	25161.198007	30.012404
408.344104	25192.542567	30.017421
408.555559	25240.716433	30.022439
409.248191	25275.208588	30.027456
409.397875	25323.101618	30.032474
409.534849	25360.701810	30.037492
410.379499	25412.808935	30.042509
410.989251	25453.747944	30.047527
411.609306	25486.918348	30.052544
412.049228	25540.959870	30.057562
412.212784	25581.646716	30.062580
412.626302	25613.648906	30.067597
413.222724	25652.820844	30.072615
413.870566	25693.520538	30.077632
413.961150	25727.241944	30.082650
414.510211	25758.490025	30.087668
414.974821	25802.309079	30.092685
415.202153	25845.691397	30.097703
415.527756	25882.232865	30.102720
416.109706	25927.910838	30.107738
416.568255	25956.272538	30.112756
417.008210	25990.811817	30.117773
417.133294	26029.533755	30.122791
417.388054	26078.379078	30.127808
418.112187	26121.153292	30.132826
418.369992	26154.286735	30.137844
419.337245	26189.255684	30.142861
419.245373	26235.652942	30.147879
419.799110	26272.766108	30.152896
420.090868	26319.052907	30.157914
420.732378	26349.156126	30.162932
421.520044	26382.093187	30.167949
421.717455	26423.528518	30.172967
421.500199	26452.710942	30.177984
422.061743	26493.684892	30.183002
422.657273	26533.206286	30.188020
423.307643	26570.203740	30.193037
423.295971	26600.776214	30.198055
423.737814	26643.336621	30.203072
424.072669	26683.006581	30.208090
424.836855	26715.025112	30.213108
425.343001	26756.457007	30.218125
425.191839	26802.087459	30.223143
425.820487	26838.058605	30.228160
426.207679	26877.221447	30.233178
426.521388	26928.821544	30.238196
427.281572	26968.223192	30.243213
427.275516	27014.084203	30.248231
427.740570	27054.088432	30.253248
428.459330	27101.277143	30.258266
428.683671	27149.396652	30.263284
429.070609	27194.425431	30.268301
429.579276	27237.684498	30.273319
430.244365	27273.739195	30.278336
430.526454	27316.300754	30.283354
431.282035	27355.533226	30.288372
431.804267	27403.543473	30.293389
431.828302	27439.913769	30.298407
432.065161	27488.885380	30.303424
433.129591	27529.416068	30.308442
433.494468	27577.306001	30.313460
433.844006	27618.448160	30.318477
433.969486	27665.174903	30.323495
434.238741	27698.340676	30.328512
434.393679	27753.311286	30.333530
435.030837	27794.573084	30.338548
435.830183	27837.642525	30.343565
436.015286	27887.685054	30.348583
436.399818	27940.553378	30.353600
437.051828	27984.208739	30.358618
437.076459	28036.716524	30.363636
438.170895	28075.044023	30.368653
438.208712	28125.135487	30.373671
438.983495	28162.388142	30.378688
439.619337	28217.436373	30.383706
439.891460	28265.418297	30.388724
440.511336	28299.573043	30.393741
440.982437	28345.520326	30.398759
441.387141	28379.241175	30.403776
441.884264	28424.697864	30.408794
442.248766	28464.391933	30.413812
442.740252	28503.800718	30.418829
442.678497	28549.838242	30.423847
443.437562	28593.326438	30.428864
444.083954	28637.786818	30.433882
443.982798	28696.959170	30.438900
445.006888	28725.691255	30.443917
445.322180	28774.622057	30.448935
445.766536	28802.642306	30.453952
446.469240	28855.564294	30.458970
446.481118	28909.624928	30.463988
447.298490	28944.337661	30.469005
447.436722	28989.112270	30.474023
448.086497	29028.762750	30.479040
448.576371	29076.775678	30.484058
448.635110	29120.109206	30.489076
449.213615	29162.628182	30.494093
450.022337	29206.109903	30.499111
450.184666	29245.261941	30.504128
450.294264	29285.275649	30.509146
451.024834	29336.620582	30.514164
451.538866	29359.649712	30.519181
451.315491	29414.266845	30.524199
452.132696	29448.714975	30.529216
452.586229	29483.441361	30.534234
452.896272	29530.920942	30.539252
453.730553	29571.447487	30.544269
454.040572	29627.106794	30.549287
454.174889	29666.245057	30.554304
454.851731	29708.281997	30.559322
455.371440	29747.360050	30.564340
455.617872	29794.793312	30.569357
456.418204	29852.544591	30.574375
456.835305	29889.565638	30.579392
457.434945	29933.935009	30.584410
457.604669	29976.279488	30.589428
458.299902	30010.867769	30.594445
458.461393	30063.049554	30.599463
458.772862	30116.680835	30.604480
459.542666	30160.006317	30.609498
459.699985	30212.404057	30.614516
460.254547	30249.189295	30.619533
460.731147	30304.350240	30.624551
460.990630	30362.706008	30.629568
461.923024	30405.810578	30.634586
462.105457	30452.269244	30.639604
462.589775	30500.134647	30.644621
463.044583	30557.606985	30.649639
463.542925	30599.035238	30.654656
464.307576	30649.284500	30.659674
464.758496	30693.792584	30.664692
465.310600	30736.805695	30.669709
465.195731	30789.159027	30.674727
465.797619	30845.774694	30.679744
466.565187	30899.621034	30.684762
466.871936	30950.530648	30.689780
468.033994	30994.308485	30.694797
468.058720	31043.005712	30.699815
468.591182	31089.385695	30.704832
469.444355	31135.273039	30.709850
469.604927	31172.842290	30.714868
470.006698	31220.690680	30.719885
470.514325	31266.265783	30.724903
471.044558	31316.047651	30.729920
471.237358	31358.049973	30.734938
471.773846	31410.517786	30.739956
472.072458	31458.250125	30.744973
472.752938	31510.904253	30.749991
473.355346	31553.051429	30.755008
473.663228	31589.953547	30.760026
473.948236	31645.432547	30.765044
474.617321	31691.153980	30.770061
475.142388	31747.442765	30.775079
475.712926	31801.360236	30.780096
476.097454	31848.637490	30.785114
476.317117	31897.255608	30.790132
476.813893	31941.677002	30.795149
477.411032	31997.601153	30.800167
477.801395	32053.968761	30.805184
478.531026	32098.429879	30.810202
479.297750	32144.446787	30.815220
479.614019	32184.490620	30.820237
480.059622	32224.735539	30.825255
480.494771	32280.540417	30.830272
481.287814	32330.846200	30.835290
481.361582	32385.013680	30.840308
481.826672	32418.383958	30.845325
482.233941	32469.199356	30.850343
482.355664	32511.322607	30.855360
483.113787	32548.901898	30.860378
483.594351	32609.954128	30.865396
483.855992	32651.227561	30.870413
484.510274	32698.173675	30.875431
484.914373	32744.002143	30.880448
485.664057	32794.202036	30.885466
485.779086	32837.951767	30.890484
486.436515	32879.473442	30.895501
486.836315	32931.770506	30.900519
487.177708	32987.275848	30.905536
487.962932	33034.448771	30.910554
488.052586	33078.462186	30.915572
488.439092	33141.307225	30.920589
489.123994	33188.236998	30.925607
489.631076	33244.425155	30.930624
490.676216	33291.905670	30.935642
491.018637	33346.868092	30.940660
491.573280	33386.465943	30.945677
492.286620	33434.738454	30.950695
492.295037	33490.392113	30.955712
492.721404	33538.577042	30.960730
493.191333	33598.059562	30.965748
493.954583	33646.229908	30.970765
494.432447	33683.001616	30.975783
494.815396	33750.850010	30.980800
495.441004	33803.019041	30.985818
495.704572	33845.609576	30.990836
496.403489	33904.146672	30.995853
497.000245	33945.351195	31.000871
497.091487	34000.961619	31.005888
497.814043	34050.745165	31.010906
497.978958	34107.071411	31.015924
498.531106	34159.404570	31.020941
499.289269	34217.794163	31.025959
499.946101	34278.583380	31.030976
500.558563	34332.045575	31.035994
500.534885	34385.993216	31.041012
501.020008	34441.233303	31.046029
501.905770	34497.137881	31.051047
501.981187	34547.175699	31.056064
502.897921	34604.694299	31.061082
503.389318	34668.153403	31.066100
503.901238	34721.809367	31.071117
504.508042	34773.136507	31.076135
505.167456	34822.381692	31.081152
505.680526	34873.534076	31.086170
506.247763	34914.353109	31.091188
506.616891	34972.666622	31.096205
506.688151	35024.603037	31.101223
507.475423	35086.467983	31.106240
507.839162	35131.599818	31.111258
508.311016	35197.156409	31.116276
508.846071	35245.227046	31.121293
509.513259	35297.570296	31.126311
510.113666	35361.943862	31.131328
510.726927	35404.893753	31.136346
511.046735	35462.154096	31.141364
511.651176	35511.194514	31.146381
512.153394	35575.957158	31.151399
512.878078	35625.244569	31.156416
513.294116	35665.943303	31.161434
514.058181	35728.275330	31.166452
514.495271	35781.224877	31.171469
514.860845	35829.563655	31.176487
515.358182	35884.849852	31.181504
516.171541	35927.997090	31.186522
516.659253	35971.726553	31.191540
516.712119	36018.736318	31.196557
517.450612	36059.486470	31.201575
517.560100	36102.598874	31.206592
518.287229	36150.034461	31.211610
519.405056	36193.918614	31.216628
519.409882	36247.777995	31.221645
519.829663	36285.726776	31.226663
520.132899	36351.129962	31.231680
520.633484	36394.599029	31.236698
521.425766	36451.060868	31.241716
521.728313	36494.093240	31.246733
522.245932	36546.943553	31.251751
522.680086	36604.739176	31.256768
523.177112	36665.825835	31.261786
523.659338	36709.867510	31.266804
524.351797	36766.560809	31.271821
525.024719	36824.458741	31.276839
525.466091	36893.724447	31.281856
525.904901	36941.795018	31.286874
526.581574	36996.910572	31.291892
526.781275	37052.202146	31.296909
527.456883	37105.174531	31.301927
528.036006	37163.448503	31.306944
528.465829	37214.524700	31.311962
529.169566	37278.875222	31.316980
529.184257	37341.683440	31.321997
530.099088	37398.792549	31.327015
530.697699	37458.126610	31.332032
531.361361	37522.180612	31.337050
531.964209	37575.614523	31.342068
532.038539	37632.995013	31.347085
532.854450	37685.529505	31.352103
533.431007	37748.541795	31.357120
533.853776	37798.988132	31.362138
534.784761	37863.854966	31.367156
534.904907	37918.845051	31.372173
535.571157	37976.898906	31.377191
535.568247	38043.025504	31.382208
536.922558	38094.597688	31.387226
537.109680	38157.096715	31.392244
537.753462	38222.439622	31.397261
538.259309	38270.464726	31.402279
538.793089	38333.251450	31.407296
539.387176	38385.854014	31.412314
539.944252	38443.787104	31.417332
540.163514	38510.923759	31.422349
540.775862	38569.816068	31.427367
541.279576	38629.617210	31.432384
542.022247	38690.892486	31.437402
542.519621	38752.250622	31.442420
542.844907	38819.004844	31.447437
543.509403	38875.278063	31.452455
544.310281	38937.221577	31.457472
544.716901	38995.407371	31.462490
545.511526	39054.032143	31.467508
545.938595	39118.836226	31.472525
546.348691	39172.645777	31.477543
546.872124	39233.273938	31.482560
547.667355	39299.266724	31.487578
548.466232	39344.921088	31.492596
549.105019	39410.489710	31.497613
549.520268	39454.863693	31.502631
550.055525	39516.477346	31.507648
550.689193	39563.403887	31.512666
551.239173	39622.757839	31.517684
551.360962	39674.488892	31.522701
551.707687	39730.289199	31.527719
552.612616	39789.455208	31.532736
553.037297	39843.447538	31.537754
553.224024	39904.206198	31.542772
553.934139	39954.713746	31.547789
554.588261	40014.052456	31.552807
554.767871	40079.846794	31.557824
555.658869	40139.724252	31.562842
556.053540	40192.324489	31.567860
556.389199	40255.723318	31.572877
557.189695	40311.700694	31.577895
557.986942	40374.610173	31.582912
558.403237	40435.125655	31.587930
558.708803	40492.369984	31.592948
559.277955	40549.174745	31.597965
559.878874	40600.023435	31.602983
560.698287	40668.495747	31.608000
561.522430	40733.293044	31.613018
561.626204	40783.827910	31.618036
562.091976	40853.924649	31.623053
562.805274	40917.614100	31.628071
563.279866	40981.847081	31.633088
564.113355	41038.466252	31.638106
564.632764	41099.973022	31.643124
565.266081	41170.392384	31.648141
566.009170	41232.958642	31.653159
566.194370	41300.014364	31.658176
566.712358	41367.157312	31.663194
567.589390	41422.980083	31.668212
568.131657	41492.516643	31.673229
568.792271	41547.323735	31.678247
569.210232	41612.908261	31.683264
569.703538	41672.713064	31.688282
570.573437	41730.416168	31.693300
570.827890	41786.546085	31.698317
571.923928	41857.318938	31.703335
572.161398	41926.442902	31.708352
573.070038	41995.088804	31.713370
573.784365	42043.323596	31.718388
574.227823	42102.675665	31.723405
574.722525	42166.137334	31.728423
575.189966	42228.686352	31.733440
575.546411	42286.762274	31.738458
576.912031	42350.562441	31.743476
576.885887	42414.580764	31.748493
577.676726	42456.662998	31.753511
578.167295	42523.699921	31.758528
578.844982	42591.099890	31.763546
579.537098	42645.702386	31.768564
580.169670	42698.454797	31.773581
580.748539	42767.002951	31.778599
581.127418	42824.545475	31.783616
581.593727	42883.826490	31.788634
582.272317	42943.023818	31.793652
583.061554	43008.478448	31.798669
583.727280	43065.160738	31.803687
583.963143	43126.616376	31.808704
584.502256	43190.788771	31.813722
585.282040	43243.917910	31.818740
585.780375	43320.298268	31.823757
586.324611	43372.952268	31.828775
586.984542	43438.036258	31.833792
587.574583	43495.844739	31.838810
587.997798	43550.371402	31.843828
588.569136	43628.253115	31.848845
589.247787	43688.666874	31.853863
589.767176	43748.865379	31.858880
589.942743	43816.404644	31.863898
591.067944	43877.463739	31.868916
591.289228	43933.420864	31.873933
592.161746	43995.727998	31.878951
592.787076	44047.428419	31.883968
593.163226	44111.122966	31.888986
593.716462	44164.232861	31.894004
594.161561	44232.819145	31.899021
594.902456	44296.804997	31.904039
595.413056	44351.066919	31.909056
596.073959	44425.407791	31.914074
596.870662	44473.913300	31.919092
597.629657	44541.110368	31.924109
598.033354	44598.969875	31.929127
598.833819	44656.666184	31.934144
599.220318	44724.523068	31.939162
600.099756	44784.414960	31.944180
600.336334	44850.695336	31.949197
600.609112	44913.725197	31.954215
601.352981	44971.817046	31.959232
601.949457	45042.754222	31.964250
602.707336	45110.301087	31.969268
602.958793	45178.515757	31.974285
603.663990	45237.114081	31.979303
604.491330	45305.763982	31.984320
604.857035	45376.485327	31.989338
605.349873	45454.341425	31.994356
606.185834	45523.534659	31.999373
606.824337	45592.018911	32.004391
607.050843	45667.330204	32.009408
607.829040	45742.454134	32.014426
608.842268	45804.174948	32.019444
609.172447	45884.310019	32.024461
609.621408	45952.103901	32.029479
610.618684	46020.058826	32.034496
610.654296	46099.083149	32.039514
611.509410	46168.129871	32.044532
612.235010	46242.510918	32.049549
612.645743	46306.921125	32.054567
613.551799	46391.212560	32.059584
613.666404	46461.476882	32.064602
614.463066	46536.341201	32.069620
615.028661	46616.891156	32.074637
615.781641	46696.918615	32.079655
616.637543	46773.001708	32.084672
617.343242	46852.328595	32.089690
617.593216	46928.051620	32.094708
618.030340	46996.869008	32.099725
618.857824	47075.000930	32.104743
619.609008	47162.292820	32.109760
619.708046	47238.223980	32.114778
620.837013	47314.392653	32.119796
621.778187	47395.759588	32.124813
622.162369	47472.209916	32.129831
622.666179	47541.923180	32.134848
622.998125	47625.859955	32.139866
623.814102	47686.585609	32.144884
624.683825	47777.498976	32.149901
625.586300	47850.661914	32.154919
626.127379	47927.861028	32.159936
626.523305	48011.245128	32.164954
627.181208	48087.540780	32.169972
627.645285	48160.526638	32.174989
628.276470	48233.954723	32.180007
629.191240	48307.401898	32.185024
629.703143	48395.014364	32.190042
630.204869	48458.448459	32.195060
630.603501	48541.581010	32.200077
631.409532	48614.989265	32.205095
632.134668	48694.104428	32.210112
632.742607	48766.095384	32.215130
633.391353	48829.918721	32.220148
634.030504	48905.656967	32.225165
634.550543	48983.021111	32.230183
635.345868	49054.110536	32.235200
635.972433	49129.554135	32.240218
636.709135	49192.213231	32.245236
637.209594	49277.920173	32.250253
637.658721	49350.241525	32.255271
638.678966	49414.754880	32.260288
639.195316	49494.386347	32.265306
639.664760	49566.553352	32.270324
640.633791	49643.798794	32.275341
640.906313	49723.532510	32.280359
641.674309	49794.090716	32.285376
642.264291	49877.438567	32.290394
642.863584	49942.810204	32.295412
643.578092	50020.792745	32.300429
644.339636	50095.712215	32.305447
645.254455	50176.080847	32.310464
645.314595	50257.469402	32.315482
646.067728	50329.100855	32.320500
646.802301	50411.732010	32.325517
647.168076	50502.627552	32.330535
648.328077	50574.892038	32.335552
648.635724	50659.349897	32.340570
649.314605	50736.897532	32.345588
650.199947	50819.095261	32.350605
650.884803	50900.122498	32.355623
651.269636	50980.115035	32.360640
652.029593	51065.345070	32.365658
652.886907	51149.876818	32.370676
653.320898	51222.358263	32.375693
653.958172	51303.710730	32.380711
654.983317	51381.522665	32.385728
655.483824	51475.165998	32.390746
656.043568	51552.912189	32.395764
656.992059	51645.290161	32.400781
657.518590	51714.095038	32.405799
658.382146	51788.124487	32.410816
658.629125	51883.669459	32.415834
659.193037	51965.307814	32.420852
660.108223	52047.878547	32.425869
660.826085	52134.498509	32.430887
661.746631	52202.085168	32.435904
662.120664	52296.017368	32.440922
662.582225	52375.724270	32.445940
663.422575	52449.316517	32.450957
664.497264	52539.938156	32.455975
664.919963	52617.715686	32.460992
665.783699	52699.809547	32.466010
666.289514	52778.403533	32.471028
667.247366	52860.736331	32.476045
667.840386	52943.322716	32.481063
668.182974	53024.790614	32.486080
668.766812	53101.759862	32.491098
669.644328	53188.883939	32.496116
670.296814	53266.488422	32.501133
670.882444	53363.017849	32.506151
671.965491	53428.019785	32.511168
672.512758	53514.981640	32.516186
673.314383	53593.943350	32.521204
673.299940	53670.546211	32.526221
674.094067	53757.444990	32.531239
675.132581	53834.237856	32.536256
675.687352	53918.845985	32.541274
675.861612	54002.900180	32.546292
676.911797	54082.286555	32.551309
677.213185	54162.878904	32.556327
678.328227	54239.357354	32.561344
678.870183	54321.773057	32.566362
679.570033	54403.664390	32.571380
680.320051	54467.683523	32.576397
680.893888	54553.816047	32.581415
681.470880	54632.569610	32.586432
682.412683	54708.614745	32.591450
682.952213	54793.981462	32.596468
683.494810	54865.292746	32.601485
683.826421	54952.502501	32.606503
684.864885	55043.430560	32.611520
685.401022	55134.956563	32.616538
685.858785	55216.388672	32.621556
686.804019	55304.465548	32.626573
687.288319	55397.513182	32.631591
687.759809	55484.272646	32.636608
688.914499	55573.469506	32.641626
689.403413	55662.226707	32.646644
690.331772	55747.896687	32.651661
690.631112	55841.202848	32.656679
691.553610	55930.038704	32.661696
692.177078	56023.434049	32.666714
692.813524	56116.580908	32.671732
693.703165	56194.474282	32.676749
694.240713	56283.662858	32.681767
695.135465	56381.548484	32.686784
695.491228	56483.044046	32.691802
696.241133	56576.554655	32.696820
697.296720	56668.511499	32.701837
697.616581	56763.425565	32.706855
698.522202	56849.033436	32.711872
699.135086	56954.224761	32.716890
699.986262	57047.423889	32.721908
700.774823	57139.057276	32.726925
701.239734	57234.336553	32.731943
702.321056	57334.000607	32.736960
703.204108	57410.816708	32.741978
703.366659	57505.074803	32.746996
704.472103	57599.147633	32.752013
705.012452	57705.935870	32.757031
705.885040	57794.710501	32.762048
706.809980	57880.964590	32.767066
707.044168	57982.112095	32.772084
708.131666	58079.778250	32.777101
708.614004	58160.381058	32.782119
709.806799	58259.107415	32.787136
710.012921	58360.488749	32.792154
710.639747	58458.013377	32.797172
711.638186	58536.555548	32.802189
712.308423	58643.878235	32.807207
712.856723	58722.605428	32.812224
714.148890	58826.147839	32.817242
714.380222	58918.679072	32.822260
715.317268	59014.226885	32.827277
715.920991	59098.016496	32.832295
717.061995	59183.462866	32.837312
717.515599	59280.454600	32.842330
718.234163	59381.139651	32.847348
719.111022	59455.507353	32.852365
719.654338	59556.669972	32.857383
720.554975	59640.263043	32.862400
721.122023	59738.099657	32.867418
721.628508	59834.104219	32.872436
722.496688	59916.222179	32.877453
723.332189	60010.580833	32.882471
723.828100	60103.967616	32.887488
724.649190	60189.885372	32.892506
725.405229	60285.517149	32.897524
726.315038	60350.824522	32.902541
726.466203	60441.557431	32.907559
727.286515	60538.053641	32.912576
728.043235	60614.994608	32.917594
728.794613	60702.197377	32.922612
729.298818	60786.527411	32.927629
730.297184	60880.851251	32.932647
731.196721	60973.178007	32.937664
732.563471	61060.431271	32.942682
732.551797	61155.933461	32.947700
733.652570	61228.220566	32.952717
734.384758	61311.434265	32.957735
734.855337	61388.707313	32.962752
735.492267	61488.059171	32.967770
736.219666	61580.864597	32.972788
737.064574	61670.037470	32.977805
737.393971	61767.248386	32.982823
738.258966	61858.248205	32.987840
739.184112	61955.999588	32.992858
739.980155	62051.663611	32.997876
740.797836	62134.480551	33.002893
741.439832	62235.955250	33.007911
741.897950	62325.121420	33.012928
742.647739	62434.904387	33.017946
743.468499	62529.585183	33.022964
744.269277	62621.173921	33.027981
745.181174	62719.132959	33.032999
745.767321	62819.643908	33.038016
746.756595	62910.697761	33.043034
746.914062	63017.151285	33.048052
747.634400	63111.963972	33.053069
748.917453	63221.812505	33.058087
749.015090	63328.593252	33.063104
750.702844	63419.014148	33.068122
751.006140	63524.775960	33.073140
751.667483	63624.056569	33.078157
752.475848	63727.543421	33.083175
752.947197	63830.589684	33.088192
754.193013	63930.571317	33.093210
754.653728	64030.897868	33.098228
755.657415	64126.651294	33.103245
756.288396	64225.198342	33.108263
757.209995	64329.163746	33.113280
757.973594	64429.887617	33.118298
758.782099	64541.721832	33.123316
760.062378	64636.927423	33.128333
760.556518	64740.499311	33.133351
761.202207	64837.951211	33.138368
762.074926	64947.808257	33.143386
762.777759	65041.972563	33.148404
763.983063	65138.052802	33.153421
764.579177	65227.758495	33.158439
764.937277	65329.815666	33.163456
765.937547	65431.019291	33.168474
766.977223	65525.417550	33.173492
767.573751	65627.172677	33.178509
768.006719	65717.500780	33.183527
769.138649	65820.477059	33.188544
770.106813	65912.228866	33.193562
770.278368	66011.772854	33.198580
771.294217	66101.593188	33.203597
771.857240	66202.247900	33.208615
772.677013	66306.034783	33.213632
773.578961	66399.761421	33.218650
774.329787	66498.317556	33.223668
775.135517	66604.285835	33.228685
776.151115	66703.877635	33.233703
776.572253	66787.481122	33.238720
777.789092	66869.035527	33.243738
778.147342	66962.064274	33.248756
779.052212	67052.145936	33.253773
779.698142	67146.681518	33.258791
780.421657	67234.126658	33.263808
781.141556	67330.310195	33.268826
781.844507	67421.608776	33.273844
782.658383	67517.569359	33.278861
783.612078	67611.406309	33.283879
783.778419	67708.982263	33.288896
784.546016	67815.442735	33.293914
785.495821	67917.082025	33.298932
786.191091	68016.919047	33.303949
787.152064	68121.742251	33.308967
787.433910	68235.827964	33.313984
788.247356	68338.699640	33.319002
789.070218	68445.249041	33.324020
790.024815	68556.641111	33.329037
790.774843	68665.507619	33.334055
791.600219	68780.555386	33.339072
792.611494	68884.696301	33.344090
793.333597	68999.932178	33.349108
794.188337	69099.780077	33.354125
795.139158	69207.205390	33.359143
795.832662	69329.298442	33.364160
796.647341	69422.498888	33.369178
797.296639	69536.577120	33.374196
797.919208	69648.184181	33.379213
799.045270	69752.994478	33.384231
799.862381	69876.292847	33.389248
800.533476	69975.090068	33.394266
801.527972	70097.893127	33.399284
802.145965	70205.608976	33.404301
803.144508	70321.193690	33.409319
803.847962	70437.167068	33.414336
804.626666	70549.241125	33.419354
805.133739	70651.859658	33.424372
806.625305	70765.152808	33.429389
807.185128	70879.301580	33.434407
807.961151	70992.910400	33.439424
809.020814	71096.267361	33.444442
809.752652	71218.318920	33.449460
810.087412	71325.247836	33.454477
810.967082	71435.840728	33.459495
811.684372	71560.429171	33.464512
813.162125	71672.740522	33.469530
813.703705	71789.340487	33.474548
814.774158	71902.691823	33.479565
815.746695	72009.776955	33.484583
816.285596	72124.035726	33.489600
817.288029	72237.145841	33.494618
818.195296	72352.842444	33.499636
818.936948	72450.415706	33.504653
820.065429	72557.086004	33.509671
820.764558	72668.991561	33.514688
821.590114	72769.389972	33.519706
822.298762	72878.343806	33.524724
823.180622	72996.897001	33.529741
823.926100	73103.578807	33.534759
824.438169	73214.325358	33.539776
825.359288	73325.970934	33.544794
826.291313	73440.249809	33.549812
827.170132	73550.990996	33.554829
827.952639	73653.527390	33.559847
828.124376	73770.206637	33.564864
829.268682	73882.642898	33.569882
830.139038	73995.122530	33.574900
830.612414	74116.632585	33.579917
831.934453	74213.589439	33.584935
832.615513	74325.720109	33.589952
833.236400	74427.018128	33.594970
834.315385	74540.265370	33.599988
834.834014	74654.031500	33.605005
835.868887	74753.061932	33.610023
836.374521	74877.395047	33.615040
837.394111	74982.787417	33.620058
838.129724	75105.464225	33.625076
838.862399	75223.949310	33.630093
839.924421	75327.677022	33.635111
840.177226	75453.952425	33.640128
841.678739	75568.949213	33.645146
842.372772	75692.293884	33.650164
843.153825	75810.951307	33.655181
844.683554	75933.444192	33.660199
845.219361	76042.931962	33.665216
846.169074	76150.771947	33.670234
846.738409	76272.314688	33.675252
847.500234	76386.164033	33.680269
848.546497	76504.364934	33.685287
849.059339	76638.154954	33.690304
849.833952	76753.675950	33.695322
850.711300	76873.387012	33.700340
851.412195	77008.593516	33.705357
852.540906	77129.583786	33.710375
853.432835	77259.390479	33.715392
854.112712	77374.916270	33.720410
855.038098	77508.139235	33.725428
855.703290	77633.967466	33.730445
856.660374	77763.196285	33.735463
857.364837	77895.176248	33.740480
858.535472	78019.647621	33.745498
859.290106	78147.769811	33.750516
860.042512	78284.216026	33.755533
861.120074	78401.926157	33.760551
862.003504	78546.460909	33.765568
863.205337	78663.911999	33.770586
863.656442	78799.711175	33.775604
864.675208	78926.579443	33.780621
865.872545	79059.273255	33.785639
866.386506	79188.578140	33.790656
867.671305	79311.453873	33.795674
868.270600	79431.751695	33.800692
868.832218	79576.810963	33.805709
870.076969	79694.703116	33.810727
870.997735	79829.407605	33.815744
872.114332	79953.224684	33.820762
872.897405	80076.689125	33.825780
873.636675	80204.151764	33.830797
874.638526	80319.943506	33.835815
875.576479	80457.840988	33.840832
876.322089	80586.368599	33.845850
877.272067	80709.670340	33.850868
877.904316	80842.385115	33.855885
879.065230	80964.704737	33.860903
879.764408	81084.715311	33.865920
880.946345	81221.615459	33.870938
881.782390	81349.207520	33.875956
882.467047	81477.913464	33.880973
883.527886	81591.395322	33.885991
884.462836	81722.103030	33.891008
885.483604	81856.788935	33.896026
886.456150	81974.505247	33.901044
887.339723	82099.293193	33.906061
888.274004	82216.585724	33.911079
889.213454	82331.698666	33.916096
889.727864	82458.535212	33.921114
890.634091	82567.851363	33.926132
891.336425	82692.366213	33.931149
892.395139	82800.126275	33.936167
893.003133	82916.712569	33.941184
893.999776	83047.214004	33.946202
895.156649	83158.317727	33.951220
895.129905	83277.805069	33.956237
896.577550	83398.329113	33.961255
897.412217	83528.186569	33.966272
898.460376	83656.059893	33.971290
899.407810	83774.826593	33.976308
900.178450	83906.038892	33.981325
900.886624	84021.524317	33.986343
902.010832	84151.301250	33.991360
902.931206	84290.132447	33.996378
903.912320	84408.491025	34.001396
904.649149	84535.960863	34.006413
905.118773	84666.906992	34.011431
906.076783	84801.692658	34.016448
907.182747	84927.497181	34.021466
907.928314	85059.174832	34.026484
909.001729	85210.429770	34.031501
909.410242	85337.105567	34.036519
910.490341	85490.020881	34.041536
911.397314	85627.225979	34.046554
912.461159	85754.561285	34.051572
913.432141	85901.654223	34.056589
914.240758	86043.033009	34.061607
914.731292	86193.117157	34.066624
915.908859	86331.512378	34.071642
916.961470	86484.158444	34.076660
917.924188	86628.747295	34.081677
919.138230	86764.148257	34.086695
920.224768	86906.666216	34.091712
921.062753	87050.275581	34.096730
922.112225	87173.450173	34.101748
922.819696	87319.260920	34.106765
924.036195	87464.612517	34.111783
924.767591	87605.694136	34.116800
925.896906	87751.301578	34.121818
926.748045	87883.456998	34.126836
927.669562	88035.067161	34.131853
928.768859	88165.043311	34.136871
929.691706	88312.941592	34.141888
930.585383	88455.066372	34.146906
932.096230	88587.882018	34.151924
932.737955	88726.296377	34.156941
933.666807	88853.007271	34.161959
934.656207	88995.461824	34.166976
935.204871	89134.500962	34.171994
936.239207	89263.237458	34.177012
937.354014	89405.839090	34.182029
938.209005	89540.485243	34.187047
939.113451	89684.109658	34.192064
939.522686	89830.942631	34.197082
941.057719	89963.367752	34.202100
941.840870	90113.045786	34.207117
942.753601	90244.213518	34.212135
943.889915	90393.001196	34.217152
944.898532	90534.243403	34.222170
946.032117	90673.502274	34.227188
946.932777	90812.557456	34.232205
947.846100	90947.099397	34.237223
948.472315	91088.556164	34.242240
949.429630	91234.651129	34.247258
950.412095	91376.573097	34.252276
951.226024	91503.173770	34.257293
952.169295	91642.213423	34.262311
953.186629	91776.844162	34.267328
954.165366	91910.176090	34.272346
955.099704	92030.220182	34.277364
955.866717	92167.046478	34.282381
956.948675	92291.732663	34.287399
957.974159	92430.281419	34.292416
958.742706	92577.578452	34.297434
959.635553	92703.005702	34.302452
960.464171	92847.290747	34.307469
961.598274	92984.646266	34.312487
962.820986	93124.117890	34.317504
963.150244	93261.144371	34.322522
964.381891	93399.284989	34.327540
965.212814	93546.944486	34.332557
966.196043	93686.658960	34.337575
967.361696	93835.420857	34.342592
968.126675	93984.791237	34.347610
969.406624	94120.138996	34.352628
970.064872	94272.772328	34.357645
971.197443	94421.466175	34.362663
972.221390	94569.049635	34.367680
973.184948	94716.009481	34.372698
974.178685	94851.747487	34.377716
975.136186	95005.909331	34.382733
975.912924	95159.504488	34.387751
977.322160	95302.607316	34.392768
978.088596	95462.670173	34.397786
979.108084	95612.604291	34.402804
980.038114	95763.199603	34.407821
981.203432	95920.540419	34.412839
981.996443	96057.950292	34.417856
982.964252	96220.330547	34.422874
984.276483	96365.342155	34.427892
985.429744	96522.396325	34.432909
986.006447	96666.624474	34.437927
987.618156	96817.054727	34.442944
988.378898	96969.076712	34.447962
989.359224	97119.366410	34.452980
990.271687	97264.660243	34.457997
991.280947	97410.522707	34.463015
992.532502	97560.734003	34.468032
993.385839	97723.051170	34.473050
994.668410	97862.319093	34.478068
995.462497	98010.360363	34.483085
996.608410	98166.815353	34.488103
997.353641	98312.824707	34.493120
998.577221	98478.307680	34.498138
999.566439	98613.504806	34.503156
1000.452387	98763.880430	34.508173
1001.615050	98913.503516	34.513191
1002.694992	99061.238675	34.518208
1003.717678	99216.653206	34.523226
1004.765480	99352.313329	34.528244
1005.673421	99499.950660	34.533261
1006.478249	99652.143322	34.538279
1007.630981	99798.108305	34.543296
1008.626153	99956.687399	34.548314
1009.163801	100101.304814	34.553332
1010.583588	100257.739777	34.558349
1011.475776	100409.909647	34.563367
1012.974194	100556.305677	34.568384
1013.710591	100703.392174	34.573402
1014.612429	100856.893796	34.578420
1015.769586	101011.281655	34.583437
1016.904706	101168.133227	34.588455
1017.778322	101302.155280	34.593472
1018.408375	101466.288492	34.598490
1019.789694	101598.533403	34.603508
1020.777051	101733.832588	34.608525
1021.800488	101883.668662	34.613543
1022.427143	102021.155454	34.618560
1023.396870	102163.850636	34.623578
1024.443786	102306.242747	34.628596
1025.658715	102455.937338	34.633613
1026.133843	102599.535943	34.638631
1027.710428	102752.497036	34.643648
1028.257431	102904.707168	34.648666
1029.464075	103056.434360	34.653684
1030.225960	103213.201963	34.658701
1031.012892	103375.671864	34.663719
1032.336645	103526.254449	34.668736
1033.286068	103686.494296	34.673754
1034.504098	103841.697324	34.678772
1035.270630	104004.236876	34.683789
1036.307902	104165.200652	34.688807
1037.891129	104322.225247	34.693824
1038.446719	104492.952926	34.698842
1039.791830	104651.575892	34.703860
1041.144792	104794.945075	34.708877
1041.806401	104969.107364	34.713895
1042.762574	105133.549965	34.718912
1043.606231	105307.152956	34.723930
1045.062777	105465.305839	34.728948
1046.035522	105627.541991	34.733965
1046.483100	105800.182464	34.738983
1047.891533	105963.619986	34.744000
1048.804285	106135.999137	34.749018
1049.885138	106300.098197	34.754036
1050.710942	106475.142785	34.759053
1051.768146	106656.948563	34.764071
1053.474575	106821.941234	34.769088
1054.663832	107001.496464	34.774106
1056.041288	107162.636778	34.779124
1056.686948	107328.470016	34.784141
1057.797106	107507.025845	34.789159
1059.376182	107667.160567	34.794176
1060.308021	107832.393486	34.799194
1061.458455	108000.408059	34.804212
1062.866974	108160.051866	34.809229
1063.648790	108313.314693	34.814247
1064.887365	108475.928481	34.819264
1065.958697	108649.398624	34.824282
1066.826821	108812.503132	34.829300
1068.154949	108977.197586	34.834317
1068.893058	109141.947148	34.839335
1070.109300	109291.354651	34.844352
1070.999378	109461.674267	34.849370
1071.890392	109627.556157	34.854388
1072.957421	109795.554400	34.859405
1074.336003	109972.330847	34.864423
1075.807610	110133.495557	34.869440
1077.053840	110291.703477	34.874458
1077.257248	110461.780361	34.879476
1078.795899	110626.703223	34.884493
1079.191997	110793.885510	34.889511
1080.861574	110951.979380	34.894528
1082.146633	111127.901215	34.899546
1083.003207	111293.238323	34.904564
1084.239093	111457.641768	34.909581
1085.178612	111630.969686	34.914599
1086.412214	111792.673791	34.919616
1087.301932	111959.594039	34.924634
1088.370580	112121.541049	34.929652
1089.969165	112291.712609	34.934669
1090.256907	112450.714289	34.939687
1091.712729	112595.634080	34.944704
1092.697995	112750.532981	34.949722
1093.475671	112921.368694	34.954740
1095.039395	113075.924783	34.959757
1095.297144	113236.545283	34.964775
1096.848321	113395.619653	34.969792
1097.743087	113555.558441	34.974810
1099.026755	113723.350999	34.979828
1100.318788	113878.295474	34.984845
1100.769609	114042.186800	34.989863
1101.609770	114216.925104	34.994880
1103.184313	114384.332731	34.999898
1104.029380	114564.309942	35.004916
1105.002229	114733.449459	35.009933
1105.678085	114910.119236	35.014951
1107.279555	115086.429338	35.019968
1108.555642	115266.520072	35.024986
1109.494838	115454.071424	35.030004
1110.495670	115623.553092	35.035021
1111.618454	115805.890026	35.040039
1112.864404	115978.911646	35.045056
1114.407398	116171.407408	35.050074
1114.985602	116351.105331	35.055092
1116.319256	116528.237919	35.060109
1117.531049	116710.819025	35.065127
1118.719637	116893.455391	35.070144
1119.651645	117074.458558	35.075162
1120.839702	117260.331153	35.080180
1122.354647	117442.944469	35.085197
1123.095340	117633.061943	35.090215
1123.923112	117811.763811	35.095232
1125.143203	118002.759396	35.100250
1126.370880	118185.040751	35.105268
1127.897769	118378.641186	35.110285
1128.751581	118568.428542	35.115303
1129.779898	118747.572741	35.120320
1131.055054	118934.581513	35.125338
1132.452074	119125.212560	35.130356
1134.063984	119310.331205	35.135373
1134.858437	119499.954899	35.140391
1136.183743	119685.500762	35.145408
1137.538789	119863.546208	35.150426
1138.333114	120046.589260	35.155444
1139.508830	120225.628494	35.160461
1140.767020	120413.217937	35.165479
1142.068287	120601.841710	35.170496
1143.326413	120777.572512	35.175514
1143.975065	120969.458802	35.180532
1145.574184	121164.482687	35.185549
1146.516223	121341.178845	35.190567
1147.760027	121530.589910	35.195584
1148.872979	121716.330953	35.200602
1149.585423	121904.355515	35.205620
1151.177322	122084.289538	35.210637
1152.526375	122278.419396	35.215655
1153.811437	122464.847419	35.220672
1154.424855	122640.966591	35.225690
1155.670879	122835.927197	35.230708
1156.968868	123004.278677	35.235725
1158.092098	123194.921757	35.240743
1159.335475	123384.494016	35.245760
1160.561351	123574.729584	35.250778
1161.394974	123767.006475	35.255796
1163.045389	123946.939788	35.260813
1163.969659	124134.459683	35.265831
1164.866244	124318.952802	35.270848
1166.351203	124504.750138	35.275866
1167.145033	124689.489392	35.280884
1168.318163	124853.047420	35.285901
1169.283469	125036.289804	35.290919
1170.240676	125213.838086	35.295936
1171.538422	125393.630083	35.300954
1172.787913	125578.898321	35.305972
1174.215663	125750.831274	35.310989
1175.263328	125935.206607	35.316007
1176.635413	126126.598472	35.321024
1177.461937	126297.587536	35.326042
1178.338250	126484.542203	35.331060
1179.485673	126675.185215	35.336077
1180.975971	126863.009683	35.341095
1181.908361	127047.801350	35.346112
1183.169631	127241.017297	35.351130
1184.304791	127440.787742	35.356148
1185.608031	127635.572157	35.361165
1186.596434	127834.238310	35.366183
1187.515143	128020.254418	35.371200
1188.993524	128210.573556	35.376218
1190.207153	128413.698523	35.381236
1191.300602	128610.220435	35.386253
1192.645341	128810.167620	35.391271
1193.733574	129015.865317	35.396288
1195.005256	129223.222754	35.401306
1196.045275	129414.986231	35.406324
1197.603725	129621.425275	35.411341
1198.861837	129832.784462	35.416359
1199.887030	130022.459512	35.421376
1201.545168	130224.610063	35.426394
1202.780932	130426.599308	35.431412
1203.732593	130630.651382	35.436429
1204.928561	130825.061277	35.441447
1206.529654	131029.711426	35.446464
1207.871302	131221.042454	35.451482
1208.743033	131439.816534	35.456500
1210.229685	131624.693684	35.461517
1211.306456	131829.911858	35.466535
1212.479553	132024.635248	35.471552
1213.971983	132228.089977	35.476570
1214.935717	132430.892480	35.481588
1215.846468	132644.730647	35.486605
1217.006494	132841.172687	35.491623
1218.202478	133045.616583	35.496640
1220.005716	133252.618329	35.501658
1221.340095	133462.562130	35.506676
1222.468859	133669.620659	35.511693
1223.806178	133868.996041	35.516711
1224.914502	134080.450078	35.521728
1226.602119	134268.796383	35.526746
1227.284963	134485.762575	35.531764
1228.376166	134679.520739	35.536781
1230.170703	134883.511402	35.541799
1231.027078	135088.982235	35.546816
1232.569614	135283.624051	35.551834
1233.707615	135497.275386	35.556852
1235.162561	135691.425092	35.561869
1236.328278	135890.493698	35.566887
1237.526953	136096.270827	35.571904
1238.867224	136294.273325	35.576922
1240.027128	136498.142194	35.581940
1241.247731	136691.051182	35.586957
1242.167887	136895.390802	35.591975
1243.546329	137110.357176	35.596992
1245.100215	137310.018377	35.602010
1246.046310	137508.925354	35.607028
1247.669412	137702.105507	35.612045
1248.587611	137906.564117	35.617063
1249.759766	138110.983870	35.622080
1251.293643	138291.909042	35.627098
1252.263755	138492.694620	35.632116
1253.536596	138686.999670	35.637133
1254.713932	138871.244309	35.642151
1255.812952	139059.169465	35.647168
1257.330347	139252.969026	35.652186
1258.166535	139446.672969	35.657204
1259.443678	139652.656622	35.662221
1260.936140	139840.954776	35.667239
1262.222047	140041.481767	35.672256
1263.338058	140234.193315	35.677274
1264.237892	140440.747070	35.682292
1265.748206	140648.855964	35.687309
1266.925206	140856.713354	35.692327
1268.197099	141057.855957	35.697344
1269.043262	141253.634287	35.702362
1270.355534	141470.306092	35.707380
1271.766960	141682.064569	35.712397
1272.993722	141903.066676	35.717415
1273.978399	142113.218594	35.722432
1275.190388	142324.693801	35.727450
1276.494772	142551.651598	35.732468
1277.986378	142775.471741	35.737485
1279.230670	142999.750433	35.742503
1280.088137	143234.485057	35.747520
1281.795942	143449.694938	35.752538
1283.190640	143676.186868	35.757556
1284.167695	143894.394065	35.762573
1285.646754	144125.393074	35.767591
1286.786334	144352.067612	35.772608
1288.453087	144573.444294	35.777626
1289.763343	144812.925674	35.782644
1290.862374	145026.206918	35.787661
1292.362140	145249.427656	35.792679
1293.717941	145478.675272	35.797696
1294.994802	145710.677782	35.802714
1296.210670	145940.482448	35.807732
1297.419139	146169.197768	35.812749
1299.123816	146398.737588	35.817767
1300.147166	146641.014001	35.822784
1301.635506	146857.592727	35.827802
1302.899296	147098.234396	35.832820
1304.370285	147319.907458	35.837837
1305.610665	147543.800689	35.842855
1306.974463	147784.772571	35.847872
1308.625283	148005.734988	35.852890
1309.769644	148235.192917	35.857908
1310.967193	148461.013370	35.862925
1312.311031	148686.545337	35.867943
1313.862100	148923.152140	35.872960
1315.458989	149152.390889	35.877978
1316.680044	149376.840711	35.882996
1317.782360	149601.094277	35.888013
1318.835138	149817.410623	35.893031
1320.485903	150050.744665	35.898048
1321.925891	150277.550297	35.903066
1323.082973	150504.096521	35.908084
1324.249234	150734.653355	35.913101
1326.308731	150963.027704	35.918119
1327.176260	151193.607850	35.923136
1328.493651	151421.135569	35.928154
1330.043048	151652.778710	35.933172
1331.327637	151870.729773	35.938189
1332.405279	152092.077910	35.943207
1333.883774	152331.909717	35.948224
1335.500572	152550.928496	35.953242
1336.755530	152769.332000	35.958260
1337.697313	152992.939090	35.963277
1339.440409	153210.480880	35.968295
1340.384307	153420.862268	35.973312
1341.920755	153634.337884	35.978330
1343.350405	153833.600971	35.983348
1344.278299	154052.390678	35.988365
1345.793696	154256.021290	35.993383
1347.236343	154477.499377	35.998400
1348.703666	154689.199877	36.003418
1349.320658	154909.082446	36.008436
1350.818906	155135.492445	36.013453
1352.179491	155352.226353	36.018471
1353.731993	155581.092311	36.023488
1354.600107	155804.772688	36.028506
1356.457382	156029.022677	36.033524
1357.535109	156262.129427	36.038541
1358.921560	156492.586373	36.043559
1360.293297	156718.958828	36.048576
1361.556643	156949.322569	36.053594
1363.061478	157179.966773	36.058612
1364.480586	157416.566473	36.063629
1365.774102	157647.702572	36.068647
1366.990617	157882.812435	36.073664
1368.580568	158120.454540	36.078682
1369.897945	158361.542515	36.083700
1371.051628	158597.261654	36.088717
1372.753778	158834.584309	36.093735
1374.237565	159076.131478	36.098752
1375.668636	159313.066780	36.103770
1377.277882	159546.674329	36.108788
1378.504292	159787.096605	36.113805
1379.743366	160022.845927	36.118823
1380.994387	160262.237861	36.123840
1382.370341	160504.607289	36.128858
1383.858097	160749.562739	36.133876
1385.047421	160995.454544	36.138893
1387.201112	161239.812533	36.143911
1388.460395	161491.598782	36.148928
1389.792136	161742.105111	36.153946
1391.429499	161978.650008	36.158964
1392.376951	162211.317277	36.163981
1394.202030	162456.467710	36.168999
1395.692458	162704.020199	36.174016
1397.241068	162941.877501	36.179034
1398.529286	163170.774956	36.184052
1399.750996	163415.744134	36.189069
1401.466075	163654.428605	36.194087
1402.789828	163893.162497	36.199104
1403.842367	164140.687380	36.204122
1405.441160	164372.930278	36.209140
1407.062231	164627.300129	36.214157
1408.187060	164854.578460	36.219175
1409.510074	165105.644944	36.224192
1411.178227	165348.494536	36.229210
1412.725203	165588.177151	36.234228
1413.831310	165831.471943	36.239245
1415.510580	166063.352556	36.244263
1416.877932	166315.737004	36.249280
1417.890741	166546.136485	36.254298
1419.555631	166799.974335	36.259316
1421.444209	167041.690804	36.264333
1422.534767	167281.361869	36.269351
1424.027088	167535.940427	36.274368
1425.415312	167773.382725	36.279386
1426.959326	168015.372325	36.284404
1427.871842	168253.804869	36.289421
1429.434334	168495.869393	36.294439
1431.143266	168756.462196	36.299456
1432.615048	168979.154164	36.304474
1433.803911	169217.191137	36.309492
1435.365564	169451.577244	36.314509
1436.763614	169670.410240	36.319527
1437.949136	169897.124054	36.324544
1439.148838	170125.169563	36.329562
1440.779528	170361.363487	36.334580
1441.927127	170589.139243	36.339597
1443.186250	170833.455655	36.344615
1445.166211	171074.853906	36.349632
1446.312495	171307.038071	36.354650
1447.736552	171547.153521	36.359668
1449.056986	171796.250434	36.364685
1450.642483	172040.430795	36.369703
1452.120252	172283.308243	36.374720
1453.407719	172533.885650	36.379738
1454.669397	172778.423788	36.384756
1456.234615	173030.571945	36.389773
1458.099944	173285.162718	36.394791
1459.361682	173538.680590	36.399808
1460.233717	173783.587615	36.404826
1462.118538	174036.273089	36.409844
1463.397016	174295.517540	36.414861
1465.244263	174549.429531	36.419879
1467.220041	174809.150618	36.424896
1468.278175	175069.955830	36.429914
1470.262119	175317.283933	36.434932
1471.564810	175580.706418	36.439949
1473.105198	175818.721515	36.444967
1474.449947	176077.224805	36.449984
1475.886437	176332.946318	36.455002
1477.664251	176585.745373	36.460020
1478.955533	176851.878442	36.465037
1481.020750	177117.154714	36.470055
1482.108733	177361.886301	36.475072
1483.351899	177620.638830	36.480090
1485.245781	177877.207740	36.485108
1486.314326	178137.639973	36.490125
1487.707642	178388.701387	36.495143
1489.663369	178662.355272	36.500160
1490.894462	178923.424753	36.505178
1492.791965	179181.089043	36.510196
1494.139634	179446.967345	36.515213
1495.431299	179693.654640	36.520231
1497.054259	179960.126329	36.525248
1498.123214	180222.901259	36.530266
1499.767142	180496.533415	36.535284
1501.436558	180765.260617	36.540301
1502.868916	181025.822175	36.545319
1504.611634	181295.580778	36.550336
1506.200066	181561.148232	36.555354
1507.949501	181822.271965	36.560372
1509.395482	182095.711272	36.565389
1511.189528	182346.416204	36.570407
1512.647610	182612.057833	36.575424
1513.927586	182875.518414	36.580442
1515.379072	183177.634830	36.585460
1516.833519	183472.563921	36.590477
1517.994590	183738.102754	36.595495
1519.650167	183998.713752	36.600512
1521.137504	184272.686149	36.605530
1523.104842	184528.169988	36.610548
1524.261414	184792.036034	36.615565
1525.935605	185059.428420	36.620583
1527.636992	185323.235988	36.625600
1528.875388	185607.258229	36.630618
1530.729187	185862.356828	36.635636
1532.694295	186128.106336	36.640653
1533.772301	186385.283390	36.645671
1535.191149	186638.978813	36.650688
1536.565216	186876.400802	36.655706
1538.517528	187120.108103	36.660724
1539.905179	187371.295613	36.665741
1541.494217	187614.349710	36.670759
1542.720499	187866.859017	36.675776
1544.220200	188115.211358	36.680794
1545.864554	188366.919799	36.685812
1547.551538	188629.798087	36.690829
1548.959903	188882.306635	36.695847
1550.349042	189132.837564	36.700864
1551.527163	189388.837687	36.705882
1553.731603	189651.942191	36.710900
1554.596237	189915.663396	36.715917
1555.888960	190188.690888	36.720935
1557.898794	190444.309202	36.725952
1558.993174	190715.971961	36.730970
1560.614737	190992.023310	36.735988
1562.166986	191263.412467	36.741005
1563.641321	191532.706193	36.746023
1565.256704	191819.911249	36.751040
1566.808365	192105.044106	36.756058
1568.474913	192382.514040	36.761076
1570.020324	192666.861758	36.766093
1571.215831	192947.759578	36.771111
1573.119544	193241.222216	36.776128
1574.365730	193520.233715	36.781146
1575.793802	193806.939253	36.786164
1577.117227	194106.692535	36.791181
1578.767081	194394.939528	36.796199
1580.437696	194701.523531	36.801216
1582.414442	195006.663266	36.806234
1584.051432	195294.482407	36.811252
1585.638170	195599.760728	36.816269
1586.876168	195908.675904	36.821287
1588.998400	196205.362304	36.826304
1590.258452	196506.807341	36.831322
1592.035997	196808.527653	36.836340
1593.550710	197107.774982	36.841357
1595.463841	197419.051761	36.846375
1597.250853	197715.717566	36.851392
1598.471885	198021.718784	36.856410
1600.038498	198317.150202	36.861428
1601.572129	198620.030104	36.866445
1603.374918	198916.695824	36.871463
1605.304051	199225.027239	36.876480
1606.712834	199539.206956	36.881498
1608.695616	199840.190010	36.886516
1610.121977	200145.960102	36.891533
1611.905547	200448.093167	36.896551
1613.881137	200752.813167	36.901568
1614.956178	201053.127665	36.906586
1616.830793	201347.627458	36.911604
1618.531540	201656.253264	36.916621
1620.067311	201949.587816	36.921639
1621.999454	202255.282610	36.926656
1623.547384	202551.054900	36.931674
1625.117598	202850.075714	36.936692
1627.027202	203149.297934	36.941709
1628.756646	203455.839379	36.946727
1630.132837	203750.776812	36.951744
1631.782105	204044.224018	36.956762
1633.175090	204346.094677	36.961780
1635.278212	204639.065322	36.966797
1636.926683	204938.509059	36.971815
1638.360754	205232.779222	36.976832
1640.134912	205533.220290	36.981850
1641.562442	205823.834322	36.986868
1643.478483	206103.652275	36.991885
1644.794834	206382.446721	36.996903
1646.660707	206653.306007	37.001920
1647.987771	206940.863529	37.006938
1650.049534	207211.413417	37.011956
1651.582141	207485.374248	37.016973
1653.255157	207768.331542	37.021991
1654.927054	208048.393400	37.027008
1655.820141	208335.944395	37.032026
1657.976279	208624.187185	37.037044
1659.334720	208917.203948	37.042061
1660.755892	209211.811647	37.047079
1662.208886	209502.223168	37.052096
1663.839485	209802.616135	37.057114
1665.311703	210105.015695	37.062132
1667.152011	210405.478145	37.067149
1668.888372	210713.629025	37.072167
1670.843416	211013.362890	37.077184
1672.130628	211326.741634	37.082202
1673.715208	211629.785766	37.087220
1675.385996	211946.483812	37.092237
1677.031407	212249.798493	37.097255
1678.904975	212559.784309	37.102272
1680.555968	212881.287686	37.107290
1682.434822	213206.617073	37.112308
1683.981119	213514.063847	37.117325
1685.659046	213841.660811	37.122343
1687.266206	214156.643521	37.127360
1688.716846	214478.916462	37.132378
1690.562058	214801.077127	37.137396
1692.506042	215128.582798	37.142413
1694.136626	215452.835295	37.147431
1695.704570	215775.776856	37.152448
1697.555232	216112.595711	37.157466
1699.347953	216441.294667	37.162484
1701.488762	216773.318101	37.167501
1702.846017	217103.000214	37.172519
1704.566135	217423.251730	37.177536
1706.057017	217757.079603	37.182554
1708.295299	218087.284983	37.187572
1709.945843	218405.947535	37.192589
1711.652607	218750.894550	37.197607
1713.455204	219070.041742	37.202624
1715.330040	219405.842797	37.207642
1716.808102	219723.720088	37.212660
1719.031727	220049.914975	37.217677
1720.509290	220385.651642	37.222695
1722.481430	220704.900057	37.227712
1724.389112	221044.126242	37.232730
1725.927406	221366.186422	37.237748
1727.826666	221692.178654	37.242765
1729.145327	222008.582898	37.247783
1731.035842	222343.950781	37.252800
1732.783146	222670.271910	37.257818
1734.543185	222999.156930	37.262836
1736.318039	223320.850344	37.267853
1737.981390	223653.205570	37.272871
1740.017338	223972.317821	37.277888
1741.721364	224303.523586	37.282906
1743.520138	224625.772317	37.287924
1745.482381	224961.027785	37.292941
1747.295906	225282.715353	37.297959
1748.948048	225604.961666	37.302976
1750.658639	225924.937866	37.307994
1752.307073	226247.769038	37.313012
1754.209630	226580.671249	37.318029
1755.663144	226894.895487	37.323047
1757.600542	227221.949240	37.328064
1759.047759	227528.146698	37.333082
1760.839024	227837.338757	37.338100
1762.096491	228143.514998	37.343117
1763.761934	228451.507234	37.348135
1765.902983	228764.378766	37.353152
1767.532145	229079.515071	37.358170
1769.214957	229394.236427	37.363188
1770.867940	229708.327255	37.368205
1772.678868	230040.480928	37.373223
1774.447405	230354.045375	37.378240
1776.071197	230681.375919	37.383258
1777.776957	230995.178576	37.388276
1779.875547	231324.797116	37.393293
1781.405874	231658.619868	37.398311
1782.903995	231981.904848	37.403328
1785.060465	232325.155755	37.408346
1786.525457	232653.145293	37.413364
1788.447933	232987.032973	37.418381
1789.850398	233332.408169	37.423399
1791.921161	233673.156667	37.428416
1793.485951	234014.111128	37.433434
1795.390836	234369.974989	37.438452
1797.189055	234714.271122	37.443469
1799.047586	235074.587348	37.448487
1800.527549	235408.644192	37.453504
1802.359722	235771.326493	37.458522
1804.164671	236126.442409	37.463540
1806.333098	236476.039320	37.468557
1808.096759	236837.105495	37.473575
1809.993697	237191.088234	37.478592
1812.015200	237555.415804	37.483610
1813.619595	237912.771451	37.488628
1815.881869	238263.672870	37.493645
1817.426235	238625.660574	37.498663
1819.289536	238986.353177	37.503680
1821.403432	239342.382701	37.508698
1822.835909	239707.587456	37.513716
1824.976930	240060.309406	37.518733
1826.346354	240427.123516	37.523751
1828.424214	240789.456900	37.528768
1830.477315	241150.498096	37.533786
1832.328270	241513.323249	37.538804
1834.652425	241879.300052	37.543821
1836.352321	242237.880053	37.548839
1838.174027	242602.003759	37.553856
1840.135550	242970.575983	37.558874
1842.051224	243326.580267	37.563892
1844.136785	243682.506607	37.568909
1845.596030	244050.164966	37.573927
1847.610387	244399.013858	37.578944
1849.591458	244763.617210	37.583962
1851.167234	245114.692810	37.588980
1853.235314	245477.350687	37.593997
1855.232725	245847.766830	37.599015
1856.866275	246207.976513	37.604032
1858.830560	246564.120158	37.609050
1860.777205	246934.034147	37.614068
1862.554590	247286.446104	37.619085
1864.543667	247640.983489	37.624103
1866.205124	248005.478435	37.629120
1868.239068	248359.600965	37.634138
1870.346598	248722.221083	37.639156
1872.169070	249077.340558	37.644173
1873.901649	249443.726588	37.649191
1875.721091	249799.378490	37.654208
1877.868989	250159.906269	37.659226
1879.786740	250510.003594	37.664244
1881.612148	250857.726820	37.669261
1883.402011	251199.841009	37.674279
1885.380994	251539.689494	37.679296
1886.997740	251873.726078	37.684314
1888.812446	252205.927433	37.689332
1890.422648	252534.578410	37.694349
1892.181195	252887.768951	37.699367
1894.316790	253236.657575	37.704384
1896.116070	253577.444072	37.709402
1897.908384	253931.338068	37.714420
1899.430029	254287.661284	37.719437
1901.338886	254629.723611	37.724455
1902.984064	254985.670112	37.729472
1905.621725	255337.040572	37.734490
1906.890656	255704.373068	37.739508
1908.866734	256070.400061	37.744525
1910.318205	256443.950659	37.749543
1912.798704	256818.380627	37.754560
1914.648706	257183.154205	37.759578
1916.063768	257568.823529	37.764596
1918.215543	257931.642688	37.769613
1919.938722	258310.428722	37.774631
1921.598257	258694.506895	37.779648
1923.943298	259078.425806	37.784666
1925.576221	259467.077817	37.789684
1927.714379	259850.036026	37.794701
1929.479014	260237.521902	37.799719
1931.809126	260631.674483	37.804736
1933.749744	261026.064471	37.809754
1935.482216	261427.546890	37.814772
1937.553994	261808.527817	37.819789
1939.766007	262202.769653	37.824807
1941.653678	262604.477579	37.829824
1943.809164	262986.381162	37.834842
1945.716304	263384.603416	37.839860
1948.057474	263772.596477	37.844877
1949.698076	264173.956242	37.849895
1951.833174	264562.334248	37.854912
1953.916383	264958.795884	37.859930
1955.859565	265357.182845	37.864948
1957.918513	265739.294755	37.869965
1959.933808	266143.636130	37.874983
1961.720944	266542.423830	37.880000
1963.957873	266932.300791	37.885018
1965.454245	267323.104837	37.890036
1967.708904	267722.474969	37.895053
1969.843790	268125.087790	37.900071
1971.823418	268522.973724	37.905088
1973.771636	268911.694146	37.910106
1975.596066	269317.271274	37.915124
1977.767518	269716.823809	37.920141
1979.799487	270115.456715	37.925159
1981.493332	270512.743909	37.930176
1983.773377	270914.813994	37.935194
1986.097974	271316.697524	37.940212
1987.749872	271719.497210	37.945229
1989.634788	272101.889948	37.950247
1991.449917	272509.155800	37.955264
1994.212563	272903.496755	37.960282
1996.124165	273303.835759	37.965300
1997.869465	273705.951286	37.970317
2000.171647	274102.568267	37.975335
2002.016514	274495.445435	37.980352
2004.130434	274890.361163	37.985370
2006.189117	275288.813740	37.990388
2008.518674	275671.882664	37.995405
2010.611187	276078.706851	38.000423
2012.146329	276470.886515	38.005440
2014.765363	276835.568708	38.010458
2016.384974	277217.217589	38.015476
2018.421079	277582.597043	38.020493
2020.765544	277942.644276	38.025511
2022.513020	278315.887274	38.030528
2024.398489	278676.790166	38.035546
2026.360676	279052.992638	38.040564
2028.147354	279412.663149	38.045581
2030.201936	279790.117261	38.050599
2032.136523	280172.032337	38.055616
2034.594975	280536.163422	38.060634
2036.272246	280922.812910	38.065652
2037.887311	281306.625928	38.070669
2039.934827	281690.242297	38.075687
2041.913300	282077.371830	38.080704
2043.903411	282457.234782	38.085722
2045.834550	282854.550518	38.090740
2048.012153	283244.842204	38.095757
2049.961590	283646.213630	38.100775
2051.663830	284055.290244	38.105792
2054.004541	284454.361190	38.110810
2055.842746	284871.207453	38.115828
2057.691420	285275.353069	38.120845
2059.911211	285699.803257	38.125863
2061.758673	286113.796483	38.130880
2064.015127	286529.322899	38.135898
2065.920225	286945.079448	38.140916
2068.366715	287363.414866	38.145933
2070.298430	287786.017849	38.150951
2072.503068	288210.454399	38.155968
2074.731181	288634.173538	38.160986
2076.818739	289053.366806	38.166004
2078.649281	289486.029566	38.171021
2080.803864	289906.349366	38.176039
2082.739637	290335.790585	38.181056
2085.349965	290765.707324	38.186074
2087.198809	291196.476568	38.191092
2089.308589	291623.317256	38.196109
2091.589333	292051.397755	38.201127
2093.225354	292486.279122	38.206144
2095.525931	292924.861899	38.211162
2097.685698	293360.264417	38.216180
2099.979469	293795.312749	38.221197
2102.353356	294235.499419	38.226215
2104.303429	294666.609019	38.231232
2106.517993	295107.448851	38.236250
2108.727903	295542.548222	38.241268
2110.653854	295977.587210	38.246285
2113.042977	296413.489834	38.251303
2114.787422	296861.143212	38.256320
2117.187778	297291.528151	38.261338
2119.415366	297729.959416	38.266356
2121.335339	298170.288698	38.271373
2123.742760	298598.809261	38.276391
2125.694668	299047.022140	38.281408
2127.654726	299482.003469	38.286426
2129.891930	299923.487810	38.291444
2131.686427	300374.557840	38.296461
2133.699459	300825.463012	38.301479
2135.944722	301269.549974	38.306496
2138.354352	301708.733442	38.311514
2140.639147	302171.871633	38.316532
2142.697520	302603.106163	38.321549
2144.682169	303047.574485	38.326567
2146.648735	303495.443486	38.331584
2149.136634	303944.166330	38.336602
2151.101769	304387.661677	38.341620
2153.320325	304833.372789	38.346637
2155.882079	305274.888704	38.351655
2157.554674	305696.588037	38.356672
2159.899112	306116.934955	38.361690
2162.074767	306538.142441	38.366708
2164.183434	306956.082415	38.371725
2166.621754	307378.384004	38.376743
2168.468303	307804.708953	38.381760
2170.681138	308208.331482	38.386778
2172.634391	308635.927083	38.391796
2174.654283	309067.163586	38.396813
2176.917250	309493.307204	38.401831
2178.989970	309933.411501	38.406848
2181.042769	310350.366820	38.411866
2182.897787	310798.061006	38.416884
2185.177115	311229.694459	38.421901
2187.388238	311679.050577	38.426919
2189.661832	312133.494175	38.431936
2192.117648	312582.828778	38.436954
2194.218359	313029.930396	38.441972
2195.998770	313477.712327	38.446989
2198.196714	313919.155810	38.452007
2200.584496	314391.655246	38.457024
2202.687167	314852.748380	38.462042
2205.127860	315301.602061	38.467060
2207.118617	315760.774692	38.472077
2209.048257	316235.991399	38.477095
2211.375829	316693.173064	38.482112
2213.593908	317173.334202	38.487130
2216.049461	317645.027620	38.492148
2217.907553	318118.865038	38.497165
2220.390484	318589.046806	38.502183
2222.358268	319077.676933	38.507200
2224.752420	319553.216707	38.512218
2226.978726	320027.635583	38.517236
2229.007290	320508.449542	38.522253
2231.466228	320998.427532	38.527271
2234.049248	321486.502700	38.532288
2236.251696	321978.209678	38.537306
2238.664787	322461.174413	38.542324
2240.879997	322942.159962	38.547341
2243.072978	323419.717930	38.552359
2245.334126	323916.061835	38.557376
2247.484359	324403.637861	38.562394
2249.695457	324893.076217	38.567412
2252.071918	325391.794755	38.572429
2254.372963	325866.465652	38.577447
2256.707972	326367.868208	38.582464
2259.368725	326855.436528	38.587482
2261.620733	327336.364715	38.592500
2263.584432	327839.735239	38.597517
2266.475688	328321.820111	38.602535
2268.490177	328812.281797	38.607552
2270.886381	329288.876088	38.612570
2273.456188	329783.805476	38.617588
2275.643673	330273.612935	38.622605
2278.210176	330754.120396	38.627623
2280.717225	331236.965158	38.632640
2282.796481	331714.441825	38.637658
2285.354591	332189.909617	38.642676
2287.188410	332672.765493	38.647693
2289.568406	333142.110115	38.652711
2292.084089	333630.910067	38.657728
2294.137959	334113.637012	38.662746
2296.935619	334579.981116	38.667764
2299.335499	335066.421317	38.672781
2301.683161	335531.631653	38.677799
2304.019663	336012.742403	38.682816
2305.845547	336481.193145	38.687834
2308.320304	336953.366574	38.692852
2310.753480	337405.501980	38.697869
2313.043150	337845.276198	38.702887
2315.473732	338301.865039	38.707904
2317.514421	338743.671063	38.712922
2319.567867	339181.614352	38.717940
2321.775708	339634.036067	38.722957
2323.985877	340082.723284	38.727975
2326.254810	340541.845142	38.732992
2328.278865	341009.394346	38.738010
2330.485160	341469.883503	38.743028
2332.419749	341938.423467	38.748045
2334.869534	342412.456090	38.753063
2337.054785	342896.186241	38.758080
2338.831351	343383.600163	38.763098
2341.549283	343868.197095	38.768116
2343.784889	344360.724269	38.773133
2346.115989	344851.175277	38.778151
2348.241220	345354.533980	38.783168
2350.649918	345855.000669	38.788186
2352.937394	346357.254007	38.793204
2355.477639	346859.688531	38.798221
2357.905724	347362.209137	38.803239
2360.487131	347880.571954	38.808256
2362.325390	348392.906523	38.813274
2364.990605	348906.295564	38.818292
2367.226416	349431.433008	38.823309
2369.578087	349943.612437	38.828327
2372.242488	350460.146765	38.833344
2374.462458	350990.358071	38.838362
2376.594615	351516.872658	38.843380
2379.110511	352051.837640	38.848397
2381.515383	352582.424873	38.853415
2384.306334	353119.839025	38.858432
2386.784765	353651.284346	38.863450
2389.303834	354183.221453	38.868468
2391.622407	354724.155599	38.873485
2394.144409	355242.587057	38.878503
2396.232956	355778.570085	38.883520
2398.853788	356326.426212	38.888538
2401.398294	356857.553389	38.893556
2403.663284	357409.578137	38.898573
2406.023524	357945.379797	38.903591
2408.864469	358476.534084	38.908608
2411.128578	359019.277612	38.913626
2413.734086	359567.965557	38.918644
2416.244260	360120.638058	38.923661
2418.779342	360654.691707	38.928679
2421.466255	361189.523211	38.933696
2424.141017	361731.013131	38.938714
2426.985367	362256.802968	38.943732
2428.888063	362810.762766	38.948749
2431.353734	363342.193901	38.953767
2434.065449	363871.042519	38.958784
2436.389397	364414.971241	38.963802
2439.263275	364943.065502	38.968820
2441.389378	365476.817280	38.973837
2444.011871	366013.193248	38.978855
2446.286781	366544.773283	38.983872
2448.750573	367091.696333	38.988890
2451.310555	367622.299541	38.993908
2453.776819	368161.827473	38.998925
2456.215772	368685.131712	39.003943
2458.891072	369214.065426	39.008960
2461.125234	369763.101589	39.013978
2464.109754	370291.257221	39.018996
2466.499554	370826.235909	39.024013
2469.076942	371352.382788	39.029031
2471.435232	371865.758630	39.034048
2473.744569	372383.693261	39.039066
2476.235237	372872.452949	39.044084
2478.694432	373371.469950	39.049101
2480.961860	373875.676311	39.054119
2483.778345	374369.070776	39.059136
2485.931648	374871.148458	39.064154
2488.423999	375372.454473	39.069172
2490.577963	375890.625660	39.074189
2492.969404	376402.720463	39.079207
2495.622427	376908.558095	39.084224
2497.789607	377430.750754	39.089242
2500.393000	377945.164142	39.094260
2502.953273	378472.366574	39.099277
2505.412442	379003.753896	39.104295
2507.900860	379528.185492	39.109312
2510.091918	380060.024082	39.114330
2512.590937	380596.692246	39.119348
2515.266153	381130.535688	39.124365
2517.882774	381670.481425	39.129383
2520.134424	382211.156863	39.134400
2522.854007	382770.692425	39.139418
2525.092478	383312.765175	39.144436
2527.561375	383865.984512	39.149453
2530.283101	384420.165364	39.154471
2532.916694	384972.904444	39.159488
2535.138092	385541.599621	39.164506
2537.625465	386110.063162	39.169524
2540.342263	386677.439767	39.174541
2542.477089	387248.591688	39.179559
2545.243415	387811.807329	39.184576
2547.537245	388395.164037	39.189594
2550.425474	388965.221959	39.194612
2553.235121	389553.231095	39.199629
2555.797513	390132.251124	39.204647
2558.248591	390712.895358	39.209664
2560.833798	391296.188617	39.214682
2563.954480	391881.156447	39.219700
2566.442852	392475.272672	39.224717
2569.474348	393041.947493	39.229735
2572.288970	393621.047786	39.234752
2574.378039	394210.525682	39.239770
2577.297603	394781.531329	39.244788
2579.964088	395360.764715	39.249805
2582.474792	395946.589912	39.254823
2585.555116	396525.628964	39.259840
2587.985879	397109.666031	39.264858
2590.522419	397686.888573	39.269876
2593.154704	398272.181504	39.274893
2595.554317	398859.014830	39.279911
2598.492559	399436.637651	39.284928
2601.000394	400016.186327	39.289946
2603.744696	400595.430454	39.294964
2606.390181	401178.522318	39.299981
2608.998119	401764.085405	39.304999
2611.911720	402336.476939	39.310016
2614.336751	402928.821046	39.315034
2617.178845	403508.077622	39.320052
2619.810075	404096.715134	39.325069
2622.479694	404680.928455	39.330087
2625.217441	405256.209230	39.335104
2627.336154	405849.587631	39.340122
2630.425081	406423.366646	39.345140
2632.890761	407000.720001	39.350157
2635.412094	407583.261642	39.355175
2638.488939	408169.799732	39.360192
2640.974202	408757.123188	39.365210
2643.256198	409327.310282	39.370228
2645.891963	409905.067282	39.375245
2648.394952	410457.583023	39.380263
2651.272476	411005.169241	39.385280
2653.582325	411566.237436	39.390298
2656.354874	412111.839125	39.395316
2658.984338	412673.587561	39.400333
2661.537852	413232.348551	39.405351
2663.851050	413786.124508	39.410368
2666.606313	414352.766992	39.415386
2668.846683	414928.529603	39.420404
2671.509190	415495.560964	39.425421
2673.749499	416075.035744	39.430439
2676.722828	416651.749876	39.435456
2679.373882	417253.181151	39.440474
2681.724525	417842.503672	39.445492
2684.385794	418432.317417	39.450509
2686.936486	419039.023738	39.455527
2689.866264	419642.669328	39.460544
2692.275731	420243.647913	39.465562
2694.656624	420862.009670	39.470580
2697.511597	421485.639060	39.475597
2700.439030	422100.389014	39.480615
2703.124601	422721.833043	39.485632
2705.709653	423367.746882	39.490650
2708.415752	423988.997488	39.495668
2711.629093	424623.750649	39.500685
2713.998333	425258.160915	39.505703
2716.788362	425891.069847	39.510720
2719.402833	426529.648627	39.515738
2722.095750	427172.491956	39.520756
2724.844467	427818.136867	39.525773
2727.816782	428467.011737	39.530791
2730.592946	429113.368632	39.535808
2732.988544	429770.935034	39.540826
2736.138866	430425.227658	39.545844
2738.988125	431076.361320	39.550861
2741.804878	431738.901125	39.555879
2744.570128	432402.336283	39.560896
2747.486631	433064.764965	39.565914
2750.180151	433722.000567	39.570932
2753.446443	434377.961968	39.575949
2755.890374	435041.710880	39.580967
2759.114330	435687.274841	39.585984
2761.733525	436362.724769	39.591002
2764.827146	437029.234089	39.596020
2767.561757	437683.649729	39.601037
2770.271164	438353.911747	39.606055
2773.739977	439013.572895	39.611072
2776.072225	439667.376631	39.616090
2778.957481	440330.114272	39.621108
2782.204642	440979.485582	39.626125
2785.059757	441643.798037	39.631143
2788.177359	442289.153247	39.636160
2790.732373	442955.233846	39.641178
2793.149137	443613.735447	39.646196
2796.356988	444262.543582	39.651213
2799.021110	444930.707787	39.656231
2802.204943	445581.846968	39.661248
2805.011818	446240.193491	39.666266
2807.622433	446896.072344	39.671284
2810.420480	447544.525188	39.676301
2813.334938	448201.975874	39.681319
2815.751519	448852.814949	39.686336
2818.584749	449517.804914	39.691354
2821.544597	450181.791103	39.696372
2824.618198	450834.121939	39.701389
2826.859075	451495.293815	39.706407
2830.043303	452157.909218	39.711424
2832.738139	452804.673488	39.716442
2835.576761	453431.702998	39.721460
2838.287882	454060.799930	39.726477
2840.969334	454699.924561	39.731495
2843.853195	455318.197209	39.736512
2846.600598	455952.975174	39.741530
2849.443581	456590.794057	39.746548
2852.150753	457216.951584	39.751565
2854.735560	457860.871437	39.756583
2857.390008	458499.911411	39.761600
2860.265151	459147.422164	39.766618
2862.924413	459794.336726	39.771636
2865.876544	460459.650689	39.776653
2868.692816	461125.515098	39.781671
2871.470711	461778.088690	39.786688
2873.935636	462440.474940	39.791706
2877.064704	463121.500899	39.796724
2879.930424	463794.568971	39.801741
2882.827765	464472.095406	39.806759
2885.793564	465158.412466	39.811776
2888.791894	465851.708507	39.816794
2891.487535	466549.815408	39.821812
2894.473422	467233.521850	39.826829
2897.325740	467929.629519	39.831847
2900.403069	468624.815289	39.836864
2903.251140	469332.213324	39.841882
2906.118257	470028.482396	39.846900
2909.046633	470729.755599	39.851917
2912.023537	471443.296138	39.856935
2914.937920	472158.882802	39.861952
2918.080096	472865.426588	39.866970
2921.407941	473588.247797	39.871988
2924.952356	474297.641188	39.877005
2927.547802	475007.403856	39.882023
2930.506732	475708.104152	39.887040
2933.362161	476433.846087	39.892058
2936.262861	477154.103461	39.897076
2939.315646	477871.128668	39.902093
2942.107243	478593.908847	39.907111
2945.243211	479317.307879	39.912128
2948.194939	480039.946542	39.917146
2951.193073	480758.311120	39.922164
2954.696934	481481.502809	39.927181
2957.375343	482208.317900	39.932199
2960.830768	482926.309908	39.937216
2964.059701	483645.664780	39.942234
2966.409074	484365.778907	39.947252
2969.910661	485088.047543	39.952269
2972.848212	485812.990557	39.957287
2975.708592	486532.822891	39.962304
2978.834564	487257.466758	39.967322
2981.580326	487982.135752	39.972340
2984.997263	488709.536744	39.977357
2988.097218	489428.439550	39.982375
2991.102424	490146.164582	39.987392
2994.305208	490871.228722	39.992410
2997.399710	491589.223785	39.997428
3001.089875	492291.126359	40.002445
3003.798538	493004.833216	40.007463
3006.536900	493721.673942	40.012480
3010.102539	494432.761366	40.017498
3012.918644	495142.622801	40.022516
3016.086220	495843.483182	40.027533
3018.865669	496557.461678	40.032551
3021.977800	497262.744410	40.037568
3024.808843	497958.723686	40.042586
3027.991656	498664.230148	40.047604
3031.298204	499373.055952	40.052621
3033.691451	500061.050147	40.057639
3037.072312	500736.827531	40.062656
3039.951459	501412.551239	40.067674
3042.997160	502071.004670	40.072692
3046.161127	502738.518825	40.077709
3049.150886	503404.972467	40.082727
3051.837324	504067.467149	40.087744
3054.819010	504739.848461	40.092762
3057.924557	505421.386957	40.097780
3060.751106	506086.734935	40.102797
3063.731080	506777.586858	40.107815
3066.320323	507458.806611	40.112832
3069.574177	508145.172027	40.117850
3072.555002	508848.499790	40.122868
3075.523321	509545.707701	40.127885
3078.474649	510248.366439	40.132903
3081.279520	510962.933494	40.137920
3084.541705	511674.827437	40.142938
3087.280803	512394.461628	40.147956
3090.568520	513115.380917	40.152973
3093.809264	513840.997108	40.157991
3096.877097	514566.350833	40.163008
3099.976356	515296.639454	40.168026
3102.571872	516040.141348	40.173044
3105.403433	516783.666604	40.178061
3108.736374	517531.949661	40.183079
3111.569702	518287.760241	40.188096
3114.907979	519045.561178	40.193114
3118.176056	519814.590307	40.198132
3121.782477	520574.374988	40.203149
3124.342804	521336.843725	40.208167
3127.332053	522112.821924	40.213184
3130.603957	522892.882182	40.218202
3133.929594	523668.868478	40.223220
3137.165182	524438.492448	40.228237
3140.403703	525232.742009	40.233255
3143.380239	526007.792398	40.238272
3146.957915	526783.557507	40.243290
3149.923587	527565.803014	40.248308
3153.219966	528355.033290	40.253325
3156.592288	529139.181208	40.258343
3159.194473	529930.936726	40.263360
3162.539474	530713.537934	40.268378
3165.593600	531525.115379	40.273396
3169.582004	532317.061569	40.278413
3172.570685	533113.082650	40.283431
3176.003592	533896.582828	40.288448
3179.845865	534693.929486	40.293466
3183.026856	535490.225520	40.298484
3186.231072	536269.700683	40.303501
3189.443984	537056.205126	40.308519
3192.420906	537850.378035	40.313536
3195.914816	538631.570949	40.318554
3198.927310	539425.137856	40.323572
3202.474549	540196.288174	40.328589
3206.057177	540994.033652	40.333607
3208.789039	541769.280065	40.338624
3212.433022	542557.432428	40.343642
3215.598978	543343.301840	40.348660
3218.797459	544127.611533	40.353677
3222.150748	544899.355643	40.358695
3225.333308	545683.619824	40.363712
3228.672583	546465.402051	40.368730
3231.550304	547244.849484	40.373748
3234.872518	548019.312994	40.378765
3238.446305	548798.703631	40.383783
3241.562710	549581.275632	40.388800
3245.091043	550369.349522	40.393818
3248.167119	551133.825801	40.398836
3251.195261	551874.445024	40.403853
3254.574459	552607.744427	40.408871
3257.500138	553344.228752	40.413888
3260.687020	554070.751533	40.418906
3263.803087	554820.049761	40.423924
3267.034651	555554.696918	40.428941
3270.036141	556299.760342	40.433959
3272.689716	557058.163280	40.438976
3276.133847	557796.147830	40.443994
3278.783419	558559.266958	40.449012
3281.987609	559323.152308	40.454029
3285.335903	560107.258664	40.459047
3288.417341	560884.991719	40.464064
3291.656207	561678.880920	40.469082
3294.935600	562470.005025	40.474100
3298.326532	563267.470126	40.479117
3301.976403	564077.011943	40.484135
3304.604255	564873.935729	40.489152
3307.661589	565679.702468	40.494170
3311.045438	566497.030489	40.499188
3314.255753	567320.186701	40.504205
3317.425428	568145.694027	40.509223
3320.703830	568971.025078	40.514240
3324.216865	569814.533499	40.519258
3327.333324	570656.489981	40.524276
3330.863854	571517.391233	40.529293
3334.760808	572346.636994	40.534311
3337.869269	573200.619739	40.539328
3341.364978	574052.525890	40.544346
3344.601319	574914.216563	40.549364
3348.014875	575771.710644	40.554381
3351.215374	576626.270736	40.559399
3354.626097	577499.243993	40.564416
3358.219452	578354.611502	40.569434
3361.574777	579228.308848	40.574452
3365.100065	580094.108226	40.579469
3368.722762	580977.229876	40.584487
3372.259849	581850.992575	40.589504
3375.894709	582718.770126	40.594522
3379.166048	583582.985986	40.599540
3382.520446	584454.120707	40.604557
3386.158960	585321.092222	40.609575
3389.633109	586204.117649	40.614592
3393.189786	587075.161876	40.619610
3396.952053	587948.803257	40.624628
3400.372840	588811.232468	40.629645
3404.001593	589671.511469	40.634663
3407.270232	590557.812836	40.639680
3411.130673	591419.065444	40.644698
3414.497439	592293.616141	40.649716
3417.668840	593154.037712	40.654733
3421.503840	594008.391627	40.659751
3424.773742	594871.956239	40.664768
3428.252610	595734.019528	40.669786
3431.846466	596608.729999	40.674804
3435.527186	597462.829991	40.679821
3439.116142	598324.165539	40.684839
3442.202466	599195.694856	40.689856
3445.494105	600056.535453	40.694874
3449.336025	600919.964940	40.699892
3452.575227	601774.681680	40.704909
3455.971798	602638.138384	40.709927
3459.619604	603501.683706	40.714944
3462.860320	604355.489220	40.719962
3466.709776	605215.017402	40.724980
3469.930356	606076.318657	40.729997
3473.376083	606923.842022	40.735015
3477.060351	607777.349637	40.740020
3480.249123	608580.129690	40.745024
3483.878450	609329.918844	40.750029
3487.142195	610037.905796	40.755034
3490.308421	610681.306395	40.760039
3492.850827	611272.864866	40.765044
3495.848286	611799.872469	40.770048
3498.959453	612279.990510	40.775053
3500.930168	612703.323312	40.780058
3503.511673	613079.252338	40.785063
3505.871550	613390.317026	40.790068
3508.653393	613649.869349	40.795072
3510.361111	613854.098272	40.800077
3511.854423	614025.166297	40.805082
3513.527124	614144.319243	40.810087
3515.440211	614229.043980	40.815092
3516.445298	614262.576257	40.820096
3518.303278	614273.632185	40.825101
3518.942935	614241.292302	40.830106
3520.188116	614167.770308	40.835111
3521.080275	614078.507671	40.840116
3522.292347	613964.001462	40.845120
3522.722257	613815.925416	40.850125
3523.760755	613646.707429	40.855130
3524.699085	613442.460527	40.860135
3524.785531	613244.691309	40.865140
3525.715833	613013.792673	40.870144
3525.835931	612768.767815	40.875149
3526.023194	612506.229006	40.880154
3526.700294	612239.507283	40.885159
3526.846022	611952.813362	40.890164
3526.842241	611656.535257	40.895168
3527.216654	611343.989818	40.900173
3527.440665	611040.208301	40.905178
3527.336043	610709.368139	40.910183
3527.418506	610398.389305	40.915188
3527.350400	610066.872493	40.920192
3527.290909	609720.741612	40.925197
3527.469286	609391.414592	40.930202
3527.854081	609047.641824	40.935207
3527.179678	608706.523651	40.940212
3527.127024	608353.693807	40.945216
3527.015504	608000.911016	40.950221
3526.995142	607649.752379	40.955226
3526.936182	607295.586642	40.960231
3526.976438	606949.596490	40.965236
3526.670411	606599.647071	40.970240
3526.738147	606244.024670	40.975245
3526.174700	605894.591748	40.980250
3526.089048	605527.562812	40.985255
3526.174787	605172.550978	40.990260
3525.768261	604817.003529	40.995264
3525.885600	604472.018820	41.000269
3525.302315	604120.427596	41.005274
3525.318948	603769.381113	41.010279
3525.185236	603425.251393	41.015284
3524.912247	603078.980362	41.020288
3524.637237	602736.751391	41.025293
3524.081145	602393.554252	41.030298
3524.407557	602053.210467	41.035303
3523.656181	601727.487195	41.040308
3523.352237	601392.575243	41.045312
3523.288285	601064.972174	41.050317
3523.031536	600742.894492	41.055322
3522.890085	600413.381215	41.060327
3522.525010	600090.899983	41.065332
3522.234126	599775.204677	41.070336
3522.529652	599461.760841	41.075341
3521.712971	599150.734116	41.080346
3521.380032	598831.112483	41.085351
3521.408831	598528.094816	41.090356
3520.975404	598211.573834	41.095360
3520.991975	597931.269127	41.100365
3520.588445	597630.796413	41.105370
3520.450253	597343.591317	41.110375
3520.366715	597050.812350	41.115380
3519.872450	596764.448259	41.120384
3519.432391	596482.123643	41.125389
3519.022986	596204.743808	41.130394
3519.034570	595923.084762	41.135399
3518.888434	595659.619880	41.140404
3518.331133	595380.789455	41.145408
3518.487941	595121.620443	41.150413
3518.039928	594862.189117	41.155418
3517.962855	594592.226901	41.160423
3517.872356	594342.141917	41.165428
3517.275036	594091.929967	41.170432
3517.647272	593827.286951	41.175437
3516.860009	593576.040848	41.180442
3516.592465	593337.479321	41.185447
3516.599485	593104.178695	41.190452
3516.391797	592866.198329	41.195456
3516.269107	592623.841678	41.200461
3516.144236	592391.948624	41.205466
3515.955194	592147.187259	41.210471
3515.578072	591937.764461	41.215476
3515.560113	591713.453966	41.220480
3515.109028	591493.314190	41.225485
3514.455108	591272.650567	41.230490
3514.888971	591059.076264	41.235495
3514.145349	590840.872498	41.240500
3514.117382	590636.579830	41.245504
3514.116006	590432.279131	41.250509
3514.100708	590241.002657	41.255514
3514.033756	590024.029252	41.260519
3513.546711	589835.725178	41.265524
3513.339333	589638.105146	41.270528
3513.839175	589437.264530	41.275533
3513.212249	589253.281059	41.280538
3513.216331	589056.368898	41.285543
3512.666688	588874.721847	41.290548
3512.586867	588689.591033	41.295552
3512.520303	588515.428568	41.300557
3512.701846	588332.305208	41.305562
3512.471238	588137.567702	41.310567
3512.592247	587976.145146	41.315572
3511.870241	587794.055935	41.320576
3511.881754	587615.406939	41.325581
3511.926745	587460.453027	41.330586
3511.971718	587279.387878	41.335591
3511.467250	587122.460398	41.340596
3511.485286	586946.455442	41.345600
3511.629940	586780.450985	41.350605
3511.311927	586630.653804	41.355610
3511.111892	586461.941980	41.360615
3511.349683	586297.068298	41.365620
3510.627475	586151.136673	41.370624
3510.253325	585995.074716	41.375629
3510.132649	585837.617662	41.380634
3510.149616	585692.516631	41.385639
3509.928027	585545.997449	41.390644
3509.759604	585398.615918	41.395648
3509.739888	585264.992883	41.400653
3509.544856	585133.350429	41.405658
3509.774525	584999.534798	41.410663
3509.456788	584870.113810	41.415668
3509.281427	584736.608908	41.420672
3509.304484	584589.788057	41.425677
3508.990937	584467.680012	41.430682
3509.341491	584333.536599	41.435687
3509.051903	584207.963162	41.440692
3508.764721	584081.936760	41.445696
3508.977308	583960.492743	41.450701
3508.294708	583836.480353	41.455706
3508.442276	583708.226147	41.460711
3508.266079	583585.986564	41.465716
3507.775475	583478.934278	41.470720
3508.405015	583370.803477	41.475725
3508.619205	583259.227322	41.480730
3508.386492	583131.477030	41.485735
3508.546474	583016.748556	41.490740
3508.404309	582899.659718	41.495744
3507.931712	582786.230935	41.500749
3507.879733	582684.015474	41.505754
3507.633892	582573.807792	41.510759
3507.759162	582461.385171	41.515764
3507.857490	582351.422277	41.520768
3507.767011	582245.147760	41.525773
3507.675500	582138.320877	41.530778
3507.505711	582035.516186	41.535783
3507.594551	581941.043116	41.540788
3507.234273	581831.347291	41.545792
3507.371320	581728.491776	41.550797
3506.953047	581627.577269	41.555802
3507.316256	581529.999306	41.560807
3507.157560	581432.903194	41.565812
3507.183652	581334.924954	41.570816
3506.922154	581235.987987	41.575821
3506.715651	581150.830417	41.580826
3506.865688	581044.657191	41.585831
3506.775502	580968.304992	41.590836
3506.792550	580868.368496	41.595840
3506.731822	580789.754044	41.600845
3506.070843	580695.738570	41.605850
3506.218899	580609.217683	41.610855
3506.111056	580521.983963	41.615860
3506.176961	580439.385840	41.620864
3506.336428	580355.318275	41.625869
3506.281367	580281.061943	41.630874
3506.085059	580194.691951	41.635879
3505.791902	580113.752201	41.640884
3505.367675	580031.729130	41.645888
3505.926690	579953.062017	41.650893
3505.812466	579886.434601	41.655898
3505.682391	579805.316669	41.660903
3505.876732	579730.817084	41.665908
3505.813888	579664.280601	41.670912
3505.647764	579582.915943	41.675917
3505.826381	579507.614948	41.680922
3505.961090	579428.609274	41.685927
3505.864552	579354.503688	41.690932
3505.464952	579278.138096	41.695936
3505.666212	579205.489459	41.700941
3505.500172	579129.186634	41.705946
3505.535650	579053.403443	41.710951
3505.309975	578995.263600	41.715956
3504.814064	578917.155303	41.720960
3505.047380	578854.479496	41.725965
3504.973911	578793.506311	41.730970
3504.881909	578719.044729	41.735975
3505.224851	578665.478440	41.740980
3505.112241	578598.241238	41.745984
3505.217248	578531.571449	41.750989
3504.734911	578468.152748	41.755994
3504.858018	578403.635963	41.760999
3504.692319	578341.471039	41.766004
3504.794020	578284.028623	41.771008
3504.426978	578218.383691	41.776013
3504.590728	578161.482645	41.781018
3504.878929	578093.628045	41.786023
3504.550439	578038.909842	41.791028
3504.292913	577988.694280	41.796032
3505.220859	577924.349846	41.801037
3504.658404	577872.125039	41.806042
3505.039442	577806.862306	41.811047
3505.132494	577741.443586	41.816052
3504.963852	577677.319320	41.821056
3505.229636	577617.691083	41.826061
3505.031641	577558.235346	41.831066
3504.780724	577491.314055	41.836071
3504.568563	577430.555752	41.841076
3504.563985	577369.513875	41.846080
3504.749654	577312.354298	41.851085
3504.932740	577253.389114	41.856090
3504.850622	577195.769217	41.861095
3504.595784	577128.846374	41.866100
3504.214587	577081.053727	41.871104
3504.548688	577013.787331	41.876109
3504.482008	576974.973851	41.881114
3504.939802	576913.957535	41.886119
3504.798894	576853.636409	41.891124
3504.708452	576794.360450	41.896128
3504.983318	576730.512561	41.901133
3504.632395	576675.339752	41.906138
3504.778298	576606.194201	41.911143
3504.863050	576557.373408	41.916148
3504.858180	576495.173097	41.921152
3504.796573	576430.523347	41.926157
3504.174847	576375.692374	41.931162
3504.212056	576323.466927	41.936167
3504.169251	576273.511092	41.941172
3504.234109	576226.999484	41.946176
3504.162595	576161.246138	41.951181
3504.141923	576123.676618	41.956186
3504.083537	576067.401648	41.961191
3504.035844	576015.890344	41.966196
3504.050754	575973.398647	41.971200
3504.291310	575918.029325	41.976205
3503.886087	575876.455743	41.981210
3503.952579	575822.317122	41.986215
3504.119210	575772.727645	41.991220
3504.114413	575728.682976	41.996224
3504.080712	575671.850348	42.001229
3503.654353	575631.583480	42.006234
3504.035451	575578.397827	42.011239
3504.272705	575544.448196	42.016244
3504.029268	575494.821270	42.021248
3504.130885	575431.444600	42.026253
3504.069836	575389.213410	42.031258
3503.975708	575341.669490	42.036263
3504.178796	575289.764490	42.041268
3503.904468	575242.649664	42.046272
3503.869498	575196.199575	42.051277
3503.807960	575158.432554	42.056282
3503.819736	575108.262346	42.061287
3503.972377	575063.989795	42.066292
3504.076352	575023.788354	42.071296
3504.255549	574967.370413	42.076301
3504.087461	574924.803035	42.081306
3503.888591	574875.818618	42.086311
3503.916500	574823.888693	42.091316
3503.530077	574787.425462	42.096320
3503.831682	574737.208297	42.101325
3504.191840	574686.680735	42.106330
3503.934179	574641.968970	42.111335
3503.863835	574598.281330	42.116340
3504.075094	574552.693174	42.121344
3504.390121	574496.552676	42.126349
3504.086927	574454.004644	42.131354
3504.225777	574398.091884	42.136359
3503.825242	574355.859730	42.141364
3503.967701	574311.033933	42.146368
3503.792987	574262.544801	42.151373
3503.669306	574220.068170	42.156378
3504.026116	574165.775877	42.161383
3503.821477	574128.328820	42.166388
3503.827505	574084.426564	42.171392
3504.032410	574029.755983	42.176397
3503.852818	573994.512189	42.181402
3503.543468	573946.845525	42.186407
3503.936212	573903.484197	42.191412
3503.657638	573854.407467	42.196416
3503.785742	573819.115024	42.201421
3503.567918	573787.990844	42.206426
3503.707816	573738.697670	42.211431
3504.024036	573700.214455	42.216436
3503.769623	573656.853004	42.221440
3503.775142	573606.125190	42.226445
3503.283359	573560.743300	42.231450
3503.675483	573516.878839	42.236455
3503.659446	573483.113149	42.241460
3503.811909	573433.967214	42.246464
3504.007944	573390.935735	42.251469
3503.606396	573354.219365	42.256474
3503.449272	573308.031502	42.261479
3503.760471	573276.973746	42.266484
3503.297869	573227.270773	42.271488
3503.715421	573190.074585	42.276493
3503.861874	573156.433053	42.281498
3503.731584	573107.129197	42.286503
3503.654214	573058.318630	42.291508
3503.894660	573020.597622	42.296512
3503.519170	572975.345741	42.301517
3503.427398	572938.780310	42.306522
3503.443380	572897.631698	42.311527
3503.494783	572857.982751	42.316532
3503.271472	572819.530720	42.321536
3503.730267	572772.190642	42.326541
3503.459356	572739.165087	42.331546
3503.553409	572689.172020	42.336551
3503.463896	572648.089176	42.341556
3503.508673	572612.103500	42.346560
3503.488259	572574.020355	42.351565
3503.398359	572539.811792	42.356570
3503.343173	572496.314402	42.361575
3503.294407	572460.894850	42.366580
3503.166612	572431.007377	42.371584
3503.418024	572387.913265	42.376589
3503.396607	572361.421251	42.381594
3503.395726	572311.290823	42.386599
3503.396891	572286.701976	42.391604
3503.535178	572249.345650	42.396608
3503.441807	572197.673567	42.401613
3503.333100	572154.885777	42.406618
3503.009253	572119.658712	42.411623
3503.164435	572089.475195	42.416628
3503.196656	572051.582802	42.421632
3503.437500	572017.421327	42.426637
3503.140075	571986.003558	42.431642
3503.240913	571946.845533	42.436647
3503.443898	571903.857527	42.441652
3503.144761	571870.633132	42.446656
3503.205174	571846.084255	42.451661
3503.000769	571810.787378	42.456666
3503.114609	571774.386794	42.461671
3503.042046	571742.983384	42.466676
3502.794013	571719.987954	42.471680
3503.054798	571687.779529	42.476685
3503.287763	571652.815258	42.481690
3502.899413	571608.011599	42.486695
3503.244387	571582.614727	42.491700
3502.966321	571549.084996	42.496704
3502.981552	571509.437011	42.501709
3502.843445	571483.613595	42.506714
3502.857039	571448.984101	42.511719
3502.912167	571419.316300	42.516724
3502.949793	571388.045241	42.521728
3503.328684	571360.183514	42.526733
3503.181586	571327.937469	42.531738
3502.938817	571289.182199	42.536743
3502.959616	571259.318608	42.541748
3503.155560	571214.723174	42.546752
3503.157116	571185.866112	42.551757
3502.955680	571159.449633	42.556762
3503.069258	571120.086037	42.561767
3503.139987	571094.078535	42.566772
3503.158679	571061.454516	42.571776
3503.286890	571028.562351	42.576781
3503.170926	571002.031773	42.581786
3503.257915	570967.038039	42.586791
3503.449451	570922.542528	42.591796
3502.894268	570897.636165	42.596800
3503.325879	570854.106599	42.601805
3502.937576	570830.127557	42.606810
3503.038916	570796.937803	42.611815
3503.457542	570759.332027	42.616820
3503.364088	570730.488669	42.621824
3503.082879	570685.815203	42.626829
3502.912184	570657.184486	42.631834
3502.813920	570619.659056	42.636839
3503.149106	570587.686845	42.641844
3503.116826	570556.775760	42.646848
3502.968454	570532.306888	42.651853
3502.947831	570491.155317	42.656858
3503.155832	570459.052063	42.661863
3503.071825	570421.774701	42.666868
3503.179448	570403.037281	42.671872
3503.008745	570373.552640	42.676877
3503.110072	570353.461011	42.681882
3503.266766	570306.308513	42.686887
3503.174682	570280.826512	42.691892
3503.181505	570245.792915	42.696896
3503.044168	570207.971105	42.701901
3502.702765	570179.968162	42.706906
3503.092711	570143.067512	42.711911
3503.216212	570110.876112	42.716916
3502.810568	570083.234308	42.721920
3503.199318	570049.595933	42.726925
3503.355431	570017.549746	42.731930
3502.922559	569985.093634	42.736935
3503.182684	569943.745635	42.741940
3502.989270	569907.387145	42.746944
3503.190670	569869.310497	42.751949
3502.925090	569847.418253	42.756954
3503.337920	569814.427917	42.761959
3503.663807	569775.779389	42.766964
3503.426047	569747.056497	42.771968
3503.332377	569700.342184	42.776973
3502.670313	569677.407367	42.781978
3502.595924	569652.272549	42.786983
3502.800338	569601.194678	42.791988
3502.733830	569579.471572	42.796993
3502.678372	569543.491903	42.801997
3502.812677	569528.914901	42.807002
3502.738748	569494.142598	42.812007
3503.038978	569463.226778	42.817012
3502.622392	569438.295566	42.822017
3502.902353	569413.054635	42.827021
3502.834218	569380.640179	42.832026
3502.791002	569350.681232	42.837031
3503.324118	569324.647625	42.842036
3502.617750	569289.220661	42.847041
3502.641921	569260.455603	42.852045
3502.438743	569241.011961	42.857050
3502.585141	569206.605899	42.862055
3502.825736	569182.525088	42.867060
3502.884239	569156.565297	42.872065
3502.799749	569128.971374	42.877069
3502.386816	569112.421407	42.882074
3502.852440	569070.586388	42.887079
3502.966163	569049.235664	42.892084
3502.520521	569016.176464	42.897089
3503.290654	568985.888635	42.902093
3502.877557	568973.153343	42.907098
3502.766076	568931.558624	42.912103
3502.948175	568903.320136	42.917108
3502.622145	568874.207292	42.922113
3503.096719	568849.336269	42.927117
3502.881313	568820.356584	42.932122
3503.159604	568782.766279	42.937127
3503.331084	568763.564437	42.942132
3503.079982	568733.636382	42.947137
3503.174538	568693.966258	42.952141
3503.096875	568662.304216	42.957146
3502.785614	568623.701228	42.962151
3503.058716	568594.744999	42.967156
3502.572199	568570.224410	42.972161
3502.850428	568538.857773	42.977165
3502.904656	568520.577409	42.982170
3503.268935	568468.766756	42.987175
3502.946295	568432.875579	42.992180
3502.897004	568412.452720	42.997185
3503.076313	568384.564783	43.002189
3502.825184	568352.075639	43.007194
3503.116046	568322.463375	43.012199
3503.268038	568290.814609	43.017204
3503.018819	568266.708062	43.022209
3503.212369	568230.384168	43.027213
3503.195406	568200.217328	43.032218
3502.902739	568157.543763	43.037223
3502.916338	568122.904230	43.042228
3502.843639	568102.233485	43.047233
3503.105028	568056.611574	43.052237
3502.826463	568038.031073	43.057242
3503.017487	567998.042277	43.062247
3503.121575	567969.813699	43.067252
3502.993386	567940.717764	43.072257
3503.114679	567900.739532	43.077261
3503.179014	567870.960723	43.082266
3503.030628	567835.191043	43.087271
3502.866469	567808.309216	43.092276
3502.338758	567781.634762	43.097281
3503.160457	567737.982226	43.102285
3502.978244	567710.600985	43.107290
3503.256095	567686.963038	43.112295
3503.235708	567650.570364	43.117300
3503.006174	567623.698326	43.122305
3503.111683	567589.143227	43.127309
3503.211369	567559.257684	43.132314
3502.997992	567527.965155	43.137319
3503.178083	567491.540639	43.142324
3502.942027	567461.155109	43.147329
3503.237891	567429.381087	43.152333
3502.929746	567406.336198	43.157338
3502.846754	567362.673071	43.162343
3502.801162	567333.110871	43.167348
3502.852320	567300.922927	43.172353
3502.708344	567265.050387	43.177357
3503.005519	567248.085506	43.182362
3502.987401	567208.026266	43.187367
3503.270913	567188.754090	43.192372
3502.990143	567158.023330	43.197377
3503.185978	567114.516491	43.202381
3503.061602	567084.765157	43.207386
3503.040350	567056.202518	43.212391
3502.990657	567012.181435	43.217396
3503.059104	566988.122963	43.222401
3502.871499	566945.378288	43.227405
3502.503734	566925.655241	43.232410
3502.751608	566893.987662	43.237415
3502.722410	566875.215691	43.242420
3502.903212	566847.825860	43.247425
3502.990316	566813.472140	43.252429
3502.605630	566793.600898	43.257434
3502.687601	566766.025504	43.262439
3503.001705	566725.661634	43.267444
3502.644856	566710.254162	43.272449
3502.605390	566668.439206	43.277453
3502.885934	566647.258787	43.282458
3502.998749	566619.879045	43.287463
3502.981206	566585.641421	43.292468
3502.764861	566562.028232	43.297473
3503.079622	566525.579625	43.302477
3502.966698	566509.531280	43.307482
3502.797839	566472.003367	43.312487
3502.641728	566435.126024	43.317492
3502.695754	566414.633276	43.322497
3502.490780	566387.453285	43.327501
3502.369442	566370.803582	43.332506
3502.644010	566327.582722	43.337511
3502.542020	566317.557234	43.342516
3502.529106	566296.723293	43.347521
3502.308053	566264.223574	43.352525
3502.728470	566243.070759	43.357530
3502.402314	566228.159918	43.362535
3502.463525	566198.527918	43.367540
3502.273890	566184.248376	43.372545
3502.504773	566148.213359	43.377549
3502.487696	566131.346182	43.382554
3502.371774	566105.607635	43.387559
3502.427179	566079.741831	43.392564
3502.381498	566063.431316	43.397569
3502.405735	566028.432393	43.402573
3502.622512	566025.837847	43.407578
3502.239618	565991.053083	43.412583
3502.195026	565973.436852	43.417588
3502.228560	565952.092946	43.422593
3502.174004	565925.641486	43.427597
3502.576194	565906.951135	43.432602
3502.286358	565886.511211	43.437607
3502.612607	565869.790817	43.442612
3502.330321	565845.583969	43.447617
3502.573231	565822.098313	43.452621
3502.633791	565796.381701	43.457626
3502.694299	565768.154571	43.462631
3502.446001	565748.310421	43.467636
3502.407541	565726.274423	43.472641
3502.511291	565702.207766	43.477645
3502.729533	565675.763301	43.482650
3502.646807	565647.257010	43.487655
3502.913801	565617.440728	43.492660
3502.429434	565589.499184	43.497665
3502.966859	565566.167812	43.502669
3502.782273	565544.405364	43.507674
3502.762156	565518.801170	43.512679
3502.674201	565490.295312	43.517684
3502.557282	565464.806554	43.522689
3502.804748	565435.695808	43.527693
3503.017211	565412.967249	43.532698
3503.013570	565384.046263	43.537703
3502.438407	565352.051247	43.542708
3502.705433	565332.627939	43.547713
3502.678744	565291.408561	43.552717
3502.836837	565278.931368	43.557722
3502.932856	565238.947909	43.562727
3503.022409	565203.183117	43.567732
3502.852516	565181.668752	43.572737
3502.946344	565135.609638	43.577741
3502.767979	565115.351778	43.582746
3502.369290	565094.726626	43.587751
3502.775672	565055.447203	43.592756
3502.586792	565039.659761	43.597761
3502.649902	565014.945273	43.602765
3502.506372	564986.898783	43.607770
3502.528053	564962.240873	43.612775
3502.546573	564934.319562	43.617780
3502.612626	564911.562701	43.622785
3503.067261	564887.339079	43.627789
3502.745565	564872.224944	43.632794
3502.456155	564845.707317	43.637799
3502.597039	564817.967451	43.642804
3502.288863	564791.502847	43.647809
3502.471881	564777.113105	43.652813
3502.816372	564742.210889	43.657818
3502.339518	564716.676332	43.662823
3502.357195	564681.724598	43.667828
3502.387250	564670.823407	43.672833
3502.433475	564637.172643	43.677837
3502.536147	564630.076344	43.682842
3502.318157	564598.425130	43.687847
3502.702428	564579.835885	43.692852
3502.820360	564556.166359	43.697857
3502.565238	564530.797590	43.702861
3502.900539	564514.274699	43.707866
3502.585528	564481.433180	43.712871
3502.565523	564456.479427	43.717876
3502.366229	564420.556529	43.722881
3502.599473	564404.200083	43.727885
3502.771687	564376.554701	43.732890
3502.427256	564364.205305	43.737895
3502.824019	564326.732689	43.742900
3502.466981	564300.375039	43.747905
3502.641439	564269.113521	43.752909
3502.435341	564246.799635	43.757914
3502.379813	564230.136577	43.762919
3502.468520	564206.521127	43.767924
3502.212295	564185.972525	43.772929
3502.272687	564156.235022	43.777933
3502.238048	564156.190184	43.782938
3501.982163	564128.862222	43.787943
3502.564904	564107.278430	43.792948
3502.318600	564081.706439	43.797953
3502.275761	564064.940728	43.802957
3502.673103	564041.126045	43.807962
3502.430340	564023.286759	43.812967
3502.572438	563991.376738	43.817972
3502.398560	563973.476390	43.822977
3502.263047	563937.240730	43.827981
3502.905667	563919.664612	43.832986
3502.294670	563900.074879	43.837991
3502.587278	563870.451000	43.842996
3502.592057	563847.350120	43.848001
3502.822024	563816.631109	43.853005
3502.733654	563792.439892	43.858010
3502.517506	563767.565548	43.863015
3502.947933	563737.718916	43.868020
3502.374368	563720.834807	43.873025
3502.770798	563685.770664	43.878029
3502.794624	563669.897896	43.883034
3502.692608	563642.494523	43.888039
3502.972945	563611.264913	43.893044
3502.604752	563581.944481	43.898049
3502.789906	563553.692506	43.903053
3502.951954	563524.590352	43.908058
3502.728042	563495.196928	43.913063
3502.822329	563468.264650	43.918068
3502.619086	563454.184761	43.923073
3502.620905	563427.417503	43.928077
3502.601476	563398.694942	43.933082
3502.365674	563372.165583	43.938087
3502.402991	563339.767968	43.943092
3502.400933	563332.084617	43.948097
3502.284703	563303.477395	43.953101
3502.516654	563283.604187	43.958106
3502.287256	563271.285869	43.963111
3502.266520	563242.563129	43.968116
3502.082038	563220.595444	43.973121
3502.042244	563205.585737	43.978125
3501.953030	563196.158208	43.983130
3502.356363	563171.687957	43.988135
3502.363919	563151.749165	43.993140
3502.006263	563122.275270	43.998145
3502.594489	563105.409530	44.003149
3502.242976	563077.591850	44.008154
3502.374246	563071.695439	44.013159
3502.504716	563033.406559	44.018164
3502.464429	563020.254874	44.023169
3502.542476	562997.040420	44.028173
3502.194581	562976.805348	44.033178
3502.292326	562956.902347	44.038183
3502.298733	562934.904284	44.043188
3502.019603	562898.286085	44.048193
3502.058696	562876.282803	44.053197
3502.369411	562867.093819	44.058202
3502.449384	562853.973369	44.063207
3502.420486	562826.757543	44.068212
3502.438534	562817.212496	44.073217
3502.470514	562786.772848	44.078221
3502.327869	562759.574648	44.083226
3502.224063	562749.697039	44.088231
3502.088586	562714.261144	44.093236
3502.309435	562711.363899	44.098241
3502.488435	562677.988079	44.103245
3502.284665	562662.350416	44.108250
3502.353696	562642.350924	44.113255
3502.599081	562620.013575	44.118260
3502.337114	562591.778959	44.123265
3502.334834	562577.566152	44.128269
3501.831946	562552.683827	44.133274
3502.060421	562536.275299	44.138279
3501.990736	562513.936779	44.143284
3501.886075	562503.155076	44.148289
3501.847125	562482.971299	44.153293
3502.292189	562475.267712	44.158298
3501.934276	562462.868185	44.163303
3502.435116	562439.486086	44.168308
3502.641128	562417.455850	44.173313
3502.547468	562402.101969	44.178317
3502.546140	562380.756987	44.183322
3502.243225	562356.847464	44.188327
3502.696161	562322.071759	44.193332
3502.513635	562303.165723	44.198337
3502.314921	562278.285489	44.203341
3502.333344	562265.374901	44.208346
3502.279743	562243.987618	44.213351
3502.720210	562213.231502	44.218356
3502.379408	562194.500708	44.223361
3502.673135	562171.351354	44.228365
3502.743362	562145.474523	44.233370
3502.424824	562120.562462	44.238375
3502.634287	562095.115779	44.243380
3502.339964	562074.067169	44.248385
3502.221334	562051.132718	44.253389
3502.318651	562029.470325	44.258394
3502.304302	562013.249704	44.263399
3502.543750	561984.483210	44.268404
3502.525019	561970.925175	44.273409
3502.156809	561949.486087	44.278413
3502.135292	561929.298634	44.283418
3502.137400	561908.052708	44.288423
3502.283084	561885.528647	44.293428
3502.362641	561861.909906	44.298433
3502.134708	561844.918824	44.303437
3502.345039	561829.064635	44.308442
3502.320392	561801.192826	44.313447
3502.418542	561785.707701	44.318452
3502.307203	561761.264750	44.323457
3502.336071	561737.050964	44.328461
3502.138884	561713.475187	44.333466
3502.350170	561710.528967	44.338471
3502.550337	561668.809322	44.343476
3502.398922	561663.508895	44.348481
3502.348866	561625.444558	44.353485
3502.298205	561615.607913	44.358490
3502.020016	561592.797966	44.363495
3502.211225	561567.252541	44.368500
3501.952175	561553.229319	44.373505
3502.359737	561535.987761	44.378509
3502.283226	561520.328682	44.383514
3502.243862	561492.257532	44.388519
3502.432971	561474.397075	44.393524
3502.082694	561446.726015	44.398529
3501.985978	561433.129323	44.403533
3502.522634	561417.424479	44.408538
3502.370854	561404.137730	44.413543
3502.393219	561380.727877	44.418548
3502.582608	561352.721090	44.423553
3502.267444	561334.135600	44.428557
3502.795066	561317.327010	44.433562
3502.144725	561280.560883	44.438567
3502.370047	561273.945669	44.443572
3502.390134	561253.348724	44.448577
3502.027739	561226.382243	44.453581
3501.996967	561215.989638	44.458586
3502.376967	561191.117090	44.463591
3502.398654	561169.063106	44.468596
3502.111797	561155.746963	44.473601
3502.269441	561131.963864	44.478605
3502.349485	561110.855004	44.483610
3502.039195	561097.341541	44.488615
3502.371881	561065.996531	44.493620
3501.945509	561044.966721	44.498625
3502.424705	561030.877695	44.503629
3502.444578	561016.810228	44.508634
3502.046808	561007.429177	44.513639
3502.429059	560974.569282	44.518644
3502.373965	560964.883476	44.523649
3502.325388	560930.835061	44.528653
3502.275459	560909.947081	44.533658
3501.921264	560887.499259	44.538663
3502.523226	560872.788090	44.543668
3502.086418	560849.097352	44.548673
3502.037001	560828.058455	44.553677
3502.585132	560813.807703	44.558682
3502.005887	560787.376423	44.563687
3502.287230	560771.559944	44.568692
3502.061945	560750.146555	44.573697
3502.257987	560735.850290	44.578701
3502.205117	560713.003414	44.583706
3502.046573	560697.556989	44.588711
3502.740687	560686.799441	44.593716
3501.894049	560669.601996	44.598721
3502.144320	560663.635547	44.603725
3502.102281	560629.585241	44.608730
3501.979784	560614.384229	44.613735
3502.065495	560593.273558	44.618740
3502.080624	560579.105848	44.623745
3502.157671	560563.120102	44.628749
3502.277011	560551.447652	44.633754
3502.064034	560537.667174	44.638759
3502.140696	560506.762559	44.643764
3502.143526	560483.203284	44.648769
3501.987036	560468.007398	44.653773
3502.134949	560427.949194	44.658778
3501.930315	560422.756992	44.663783
3502.061090	560416.105848	44.668788
3501.984609	560390.800656	44.673793
3501.785530	560382.342459	44.678797
3502.037575	560369.343040	44.683802
3501.895277	560343.194082	44.688807
3502.105003	560340.750093	44.693812
3501.869589	560326.520783	44.698817
3501.553536	560301.001687	44.703821
3502.157123	560287.394661	44.708826
3502.231364	560272.664782	44.713831
3502.185485	560254.135955	44.718836
3502.182024	560237.057228	44.723841
3501.895325	560219.068324	44.728845
3501.750134	560205.678727	44.733850
3501.997198	560204.384237	44.738855
3502.096517	560177.845509	44.743860
3502.082045	560164.485663	44.748865
3501.951429	560152.450028	44.753869
3502.201370	560121.868953	44.758874
3501.985920	560106.932987	44.763879
3502.178032	560094.394738	44.768884
3502.080412	560079.992888	44.773889
3502.261056	560061.629283	44.778893
3502.028269	560036.046364	44.783898
3501.896408	560032.600799	44.788903
3502.856680	560007.233179	44.793908
3502.401579	559987.009716	44.798913
3502.155525	559962.684565	44.803917
3502.275837	559950.810434	44.808922
3502.115635	559936.066552	44.813927
3502.858545	559911.385755	44.818932
3502.290347	559884.649315	44.823937
3502.287788	559860.537062	44.828941
3502.239766	559845.423887	44.833946
3502.015907	559825.515640	44.838951
3502.274821	559804.878834	44.843956
3502.419016	559784.460866	44.848961
3502.351743	559769.501309	44.853965
3502.283165	559742.334796	44.858970
3502.202248	559729.386728	44.863975
3502.346332	559705.703351	44.868980
3502.229708	559683.115628	44.873985
3502.305639	559663.260712	44.878989
3502.358452	559636.476864	44.883994
3502.078135	559625.770222	44.888999
3502.067614	559600.151613	44.894004
3502.076320	559597.085832	44.899009
3502.243696	559574.754919	44.904013
3502.660619	559555.348875	44.909018
3502.331739	559538.922844	44.914023
3502.287725	559509.692280	44.919028
3501.987629	559480.150024	44.924033
3502.172163	559463.593390	44.929037
3502.279502	559451.519843	44.934042
3502.029930	559429.002654	44.939047
3502.277394	559404.247548	44.944052
3502.559873	559396.617622	44.949057
3502.259004	559381.694093	44.954061
3502.378845	559346.358869	44.959066
3502.138917	559336.801098	44.964071
3502.375737	559311.545093	44.969076
3502.161193	559297.411754	44.974081
3502.592121	559278.756625	44.979085
3502.324750	559263.074153	44.984090
3502.402494	559247.438182	44.989095
3502.226338	559221.894886	44.994100
3501.948917	559201.039451	44.999105
3502.352427	559176.209238	45.004109
3502.193566	559159.655626	45.009114
3502.129952	559136.505959	45.014119
3502.589086	559125.934455	45.019124
3502.235368	559114.736446	45.024129
3502.108085	559095.163537	45.029133
3502.073242	559070.250916	45.034138
3502.209260	559054.856772	45.039143
3501.987803	559024.045132	45.044148
3501.439938	559007.200452	45.049153
3501.776221	558996.547561	45.054157
3501.982006	558992.395810	45.059162
3502.005394	558983.499927	45.064167
3502.116461	558950.023714	45.069172
3501.987544	558948.536675	45.074177
3502.304521	558925.075906	45.079181
3502.086236	558903.607839	45.084186
3502.247038	558892.680856	45.089191
3502.755755	558864.869458	45.094196
3502.251847	558849.876521	45.099201
3502.367014	558818.660051	45.104205
3502.201916	558798.891609	45.109210
3502.301100	558786.567464	45.114215
3502.205213	558766.084799	45.119220
3502.272509	558739.095704	45.124225
3502.276920	558724.575776	45.129229
3502.260908	558695.991943	45.134234
3502.617368	558690.309345	45.139239
3502.283800	558664.086101	45.144244
3502.094514	558640.402476	45.149249
3502.176927	558627.628630	45.154253
3502.369445	558602.076605	45.159258
3502.032991	558586.856197	45.164263
3501.622554	558559.238016	45.169268
3501.752167	558561.880447	45.174273
3501.695701	558553.197685	45.179277
3502.122820	558528.211708	45.184282
3501.952725	558523.666393	45.189287
3501.855726	558509.764941	45.194292
3501.846093	558480.626948	45.199297
3502.137605	558468.875295	45.204301
3502.175882	558451.988433	45.209306
3502.111834	558431.449972	45.214311
3502.311430	558416.145544	45.219316
3502.323065	558401.121685	45.224321
3502.065809	558399.202471	45.229325
3502.070422	558366.846558	45.234330
3502.270902	558340.187424	45.239335
3502.095464	558324.539578	45.244340
3501.972717	558304.612969	45.249345
3501.927078	558294.320605	45.254349
3501.934676	558285.627633	45.259354
3502.030593	558257.175971	45.264359
3502.032532	558241.500287	45.269364
3501.928362	558235.839242	45.274369
3501.749306	558224.814051	45.279373
3501.939495	558202.175544	45.284378
3502.079573	558197.832823	45.289383
3502.079346	558173.415327	45.294388
3502.001154	558161.118265	45.299393
3501.698896	558145.490009	45.304397
3502.122403	558120.754953	45.309402
3501.820213	558109.346969	45.314407
3501.799208	558103.823586	45.319412
3501.969910	558075.711495	45.324417
3501.886635	558072.709942	45.329421
3502.194082	558047.389972	45.334426
3501.722319	558034.350427	45.339431
3501.758989	558020.678718	45.344436
3501.906734	558011.461212	45.349441
3501.923860	557999.400293	45.354445
3501.929270	557967.193897	45.359450
3501.771601	557974.403209	45.364455
3501.552966	557951.024254	45.369460
3501.768966	557922.954964	45.374465
3501.552636	557921.983888	45.379469
3502.187056	557912.941439	45.384474
3501.753972	557899.242541	45.389479
3501.866353	557878.826274	45.394484
3502.101295	557873.011556	45.399489
3501.591904	557865.504446	45.404493
3501.959820	557842.134067	45.409498
3501.970701	557848.663945	45.414503
3501.750233	557831.565437	45.419508
3501.918521	557803.051134	45.424513
3501.966005	557796.512034	45.429517
3502.181450	557784.369652	45.434522
3501.905882	557758.939238	45.439527
3502.100903	557747.553664	45.444532
3502.088409	557729.367381	45.449537
3501.919080	557709.346569	45.454541
3501.877897	557691.013982	45.459546
3501.996848	557688.834864	45.464551
3502.104846	557668.469166	45.469556
3501.953540	557658.594723	45.474561
3501.845254	557648.964766	45.479565
3502.115654	557615.811602	45.484570
3501.895805	557616.649840	45.489575
3501.848178	557579.828225	45.494580
3502.057541	557572.007587	45.499585
3501.539409	557564.551896	45.504589
3501.623371	557545.194632	45.509594
3502.109959	557534.617431	45.514599
3502.215771	557518.623090	45.519604
3502.328171	557502.527209	45.524609
3501.724810	557488.603233	45.529613
3502.071082	557474.530785	45.534618
3501.890432	557457.978208	45.539623
3501.859233	557443.211061	45.544628
3502.053371	557423.132947	45.549633
3502.033490	557419.719360	45.554637
3502.188395	557393.567685	45.559642
3501.862891	557386.081767	45.564647
3501.954067	557360.140962	45.569652
3502.076795	557351.278574	45.574657
3502.155667	557325.540599	45.579661
3502.041226	557305.560773	45.584666
3501.858462	557305.438572	45.589671
3501.932021	557281.610660	45.594676
3501.833505	557264.643010	45.599681
3501.993218	557255.021084	45.604685
3502.210051	557230.517478	45.609690
3501.999505	557211.004731	45.614695
3502.156989	557201.483602	45.619700
3502.345033	557177.034633	45.624705
3502.211344	557167.659489	45.629709
3502.216121	557143.691316	45.634714
3501.815920	557141.794243	45.639719
3502.082677	557113.313146	45.644724
3502.016459	557091.014093	45.649729
3502.033446	557087.946372	45.654733
3502.031235	557067.496385	45.659738
3502.044546	557050.862675	45.664743
3501.888271	557041.340222	45.669748
3502.400765	557006.841111	45.674753
3502.193307	556998.582793	45.679757
3502.010647	556983.436781	45.684762
3501.997259	556973.138234	45.689767
3502.135137	556956.635659	45.694772
3502.359847	556930.321318	45.699777
3502.259313	556919.131901	45.704781
3502.234617	556900.946263	45.709786
3501.659481	556876.766730	45.714791
3501.757776	556860.119468	45.719796
3502.105215	556855.040381	45.724801
3501.775442	556833.435265	45.729805
3502.310002	556823.653898	45.734810
3501.944276	556805.973657	45.739815
3501.856617	556775.135276	45.744820
3502.370212	556750.634543	45.749825
3502.114426	556681.282078	45.754829
3502.381700	556569.839718	45.759834
3502.175787	556415.557546	45.764839
3501.550723	556194.908415	45.769844
3501.105634	555942.016109	45.774849
3500.827692	555638.086187	45.779853
3500.495129	555278.676845	45.784858
3499.813670	554891.067680	45.789863
3499.583037	554443.720081	45.794868
3499.043245	553960.167169	45.799873
3497.947846	553433.054675	45.804877
3497.554067	552856.198958	45.809882
3496.696702	552231.283125	45.814887
3495.758758	551567.087343	45.819892
3494.817728	550860.275156	45.824897
3493.319770	550112.584908	45.829901
3492.820476	549313.659982	45.834906
3490.794164	548489.780645	45.839911
3490.086488	547623.098299	45.844916
3488.983882	546700.947635	45.849921
3487.474782	545761.289643	45.854925
3486.100961	544761.132371	45.859930
3484.362041	543730.418770	45.864935
3482.773956	542653.415805	45.869940
3481.446535	541556.205678	45.874945
3479.482047	540422.521226	45.879949
3477.654097	539244.130609	45.884954
3475.407091	538040.332469	45.889959
3473.645472	536801.718097	45.894964
3472.067085	535527.821774	45.899969
3469.699061	534242.092640	45.904973
3467.757837	532899.279427	45.909978
3465.396968	531545.365871	45.914983
3463.328556	530149.470972	45.919988
3461.126146	528728.871937	45.924993
3458.385314	527286.445213	45.929997
3456.289457	525825.424664	45.935002
3453.843005	524348.580255	45.940007
3451.230861	522829.427692	45.945012
3448.657692	521284.700910	45.950017
3445.804732	519724.621601	45.955021
3443.198875	518150.514288	45.960026
3440.348597	516553.933359	45.965031
3437.691079	514938.735812	45.970036
3435.111250	513304.177942	45.975041
3432.154324	511655.518832	45.980045
3428.987872	509987.836735	45.985050
3425.911770	508301.633993	45.990055
3422.974098	506607.894104	45.995060
3420.392444	504900.023393	46.000065
3417.136843	503171.620102	46.005069
3414.243874	501425.442790	46.010074
3410.869071	499683.117166	46.015079
3407.415406	497913.138667	46.020084
3404.327347	496133.349147	46.025089
3401.003054	494352.322079	46.030093
3398.089257	492546.580197	46.035098
3394.624285	490750.200335	46.040103
3391.495755	488935.221551	46.045108
3388.299227	487108.318651	46.050113
3384.689889	485281.514893	46.055117
3381.103631	483429.634878	46.060122
3377.766692	481594.017461	46.065127
3373.887046	479744.019401	46.070132
3370.725463	477894.197453	46.075137
3367.240381	476044.463496	46.080141
3363.907277	474169.621306	46.085146
3360.328094	472301.172109	46.090151
3356.437864	470428.006313	46.095156
3353.277507	468550.416365	46.100161
3349.522119	466667.446466	46.105165
3345.971113	464786.912459	46.110170
3342.299926	462902.241030	46.115175
3338.390061	461017.953612	46.120180
3335.214260	459123.325392	46.125185
3331.251135	457237.112816	46.130189
3327.710703	455345.062386	46.135194
3323.946549	453451.374661	46.140199
3320.228491	451549.276483	46.145204
3316.852019	449646.769851	46.150209
3312.659538	447759.732315	46.155213
3308.901806	445849.644982	46.160218
3304.893139	443961.070890	46.165223
3301.260468	442070.269479	46.170228
3297.468018	440182.339893	46.175233
3293.575250	438296.768885	46.180237
3289.872216	436402.773705	46.185242
3286.109806	434516.301217	46.190247
3282.430452	432626.692498	46.195252
3278.807718	430742.415121	46.200257
3274.771895	428868.917774	46.205261
3270.989081	426977.920775	46.210266
3267.354787	425106.034489	46.215271
3263.625250	423232.469082	46.220276
3259.375309	421352.881517	46.225281
3255.490058	419492.636821	46.230285
3251.820275	417614.191266	46.235290
3247.893600	415750.172355	46.240295
3244.072791	413893.073578	46.245300
3240.453892	412023.102422	46.250305
3236.220900	410172.747161	46.255309
3232.619225	408313.107081	46.260314
3228.731226	406471.112087	46.265319
3224.519162	404628.305662	46.270324
3221.121098	402789.280933	46.275329
3216.953685	400953.323826	46.280333
3213.223101	399119.283780	46.285338
3208.984112	397294.669871	46.290343
3205.423509	395467.372278	46.295348
3201.660408	393641.539815	46.300353
3197.611728	391830.233948	46.305357
3193.967031	390013.348716	46.310362
3190.260504	388200.248605	46.315367
3186.324423	386381.873235	46.320372
3182.655391	384581.173959	46.325377
3178.554829	382785.950296	46.330381
3175.001556	380989.881185	46.335386
3170.528115	379199.673143	46.340391
3166.964551	377412.401360	46.345396
3163.328612	375628.272274	46.350401
3159.292670	373872.764770	46.355405
3156.163025	372078.493661	46.360410
3152.096494	370306.277577	46.365415
3147.831096	368544.955498	46.370420
3144.180143	366764.855750	46.375425
3139.949726	365005.342379	46.380429
3136.816241	363256.146941	46.385434
3132.607775	361505.338653	46.390439
3128.893205	359761.923438	46.395444
3124.979860	358002.275428	46.400449
3120.977547	356266.837610	46.405453
3117.101126	354530.291884	46.410458
3113.222294	352804.860254	46.415463
3109.247735	351069.334932	46.420468
3105.462778	349351.354530	46.425473
3101.467405	347632.656094	46.430477
3098.228041	345929.106583	46.435482
3094.479629	344227.305012	46.440487
3090.543069	342532.440479	46.445492
3086.713117	340829.772059	46.450497
3082.819983	339131.939010	46.455501
3079.153934	337431.396041	46.460506
3075.409385	335742.840057	46.465511
3071.528970	334059.289028	46.470516
3067.682173	332376.521815	46.475521
3064.071057	330701.629747	46.480525
3060.506607	329021.392673	46.485530
3056.494249	327358.221751	46.490535
3052.545351	325691.791935	46.495540
3048.655167	324022.893306	46.500545
3045.016559	322363.936571	46.505549
3041.362405	320711.912936	46.510554
3037.795415	319056.122768	46.515559
3033.902445	317410.090508	46.520564
3029.622565	315765.329731	46.525569
3026.383848	314135.027591	46.530573
3022.380160	312497.204472	46.535578
3018.993998	310868.337200	46.540583
3015.066936	309244.537388	46.545588
3011.353616	307605.432024	46.550593
3007.277003	305976.941416	46.555597
3003.503572	304359.370630	46.560602
2999.959276	302749.552033	46.565607
2996.250361	301138.030223	46.570612
2992.780296	299523.495835	46.575617
2988.981021	297919.248390	46.580621
2985.440322	296311.631238	46.585626
2981.505024	294711.285239	46.590631
2977.615721	293119.084923	46.595636
2974.235578	291515.027931	46.600641
2970.014890	289929.923588	46.605645
2966.286565	288328.308373	46.610650
2962.492837	286754.284958	46.615655
2959.033342	285168.003116	46.620660
2955.269742	283595.785019	46.625665
2950.967043	282027.180206	46.630669
2947.757198	280441.719742	46.635674
2943.768087	278876.257020	46.640679
2940.173629	277312.304452	46.645684
2936.572383	275745.597459	46.650689
2932.696969	274193.110608	46.655693
2929.041265	272634.907967	46.660698
2925.475450	271086.491671	46.665703
2922.029053	269539.175661	46.670708
2918.455894	267989.281747	46.675713
2914.570819	266450.106301	46.680717
2910.797116	264902.944754	46.685722
2907.113324	263361.169891	46.690727
2903.438669	261836.050967	46.695732
2899.878519	260292.303708	46.700737
2895.820838	258763.154689	46.705741
2892.143384	257229.419594	46.710746
2888.585154	255708.431495	46.715751
2884.826464	254189.876843	46.720756
2881.168638	252666.935302	46.725761
2877.411115	251145.547304	46.730765
2873.738361	249630.243540	46.735770
2870.138573	248124.643255	46.740775
2866.202693	246631.383740	46.745780
2862.622877	245113.989794	46.750785
2859.209310	243610.769837	46.755789
2855.558518	242114.962625	46.760794
2851.985270	240614.473373	46.765799
2847.810131	239125.683432	46.770804
2844.644424	237625.853037	46.775809
2840.443124	236139.421535	46.780813
2837.212810	234656.245132	46.785818
2833.569760	233165.996956	46.790823
2829.856831	231681.969850	46.795828
2826.233274	230193.901225	46.800833
2822.381632	228723.719400	46.805837
2819.145596	227240.628553	46.810842
2815.356519	225766.359036	46.815847
2811.692295	224290.872694	46.820852
2807.904883	222814.514735	46.825857
2803.840051	221354.934625	46.830861
2800.588004	219882.978875	46.835866
2796.686230	218428.420998	46.840871
2793.133081	216962.605857	46.845876
2789.688128	215500.190986	46.850881
2785.799852	214053.921301	46.855885
2782.240253	212599.787113	46.860890
2778.518398	211152.637749	46.865895
2774.799506	209707.558098	46.870900
2771.509997	208254.524124	46.875905
2767.592783	206820.188758	46.880909
2764.112759	205371.812477	46.885914
2760.241191	203924.679166	46.890919
2756.520411	202498.594793	46.895924
2752.852583	201058.786640	46.900929
2748.841113	199637.737309	46.905933
2745.456647	198209.573758	46.910938
2742.057737	196790.492064	46.915943
2738.302360	195362.465103	46.920948
2735.095854	193938.136199	46.925953
2731.155075	192529.369923	46.930957
2727.358866	191104.579195	46.935962
2723.849446	189691.270825	46.940967
2719.959021	188272.182543	46.945972
2716.633676	186858.982807	46.950977
2713.126212	185453.978855	46.955981
2709.399441	184047.398766	46.960986
2705.608852	182648.029307	46.965991
2701.831815	181241.701299	46.970996
2698.587990	179837.195451	46.976001
2694.950695	178435.446621	46.981005
2691.234946	177041.116520	46.986010
2687.595552	175645.651677	46.991015
2683.808166	174254.409241	46.996020
2680.356625	172858.810173	47.001025
2676.321472	171475.039005	47.006029
2672.991550	170083.353944	47.011034
2669.492467	168701.790586	47.016039
2665.610373	167320.428144	47.021044
2662.409793	165942.919466	47.026049
2658.697217	164563.787327	47.031053
2654.862744	163184.447967	47.036058
2651.277931	161816.884860	47.041063
2647.649004	160442.739173	47.046068
2643.973053	159063.934309	47.051073
2640.285578	157695.776747	47.056077
2636.550281	156324.564966	47.061082
2632.851685	154962.097084	47.066087
2629.468432	153604.855188	47.071092
2626.086242	152236.102792	47.076097
2622.010710	150877.825808	47.081101
2618.686048	149518.803286	47.086106
2614.550715	148176.013863	47.091111
2611.169522	146828.050579	47.096116
2608.211821	145485.718440	47.101121
2604.327735	144057.677662	47.106125
2600.839384	142690.359459	47.111130
2597.166995	141350.921572	47.116135
2593.021881	140007.599456	47.121140
2589.690297	138662.839198	47.126145
2585.845982	137324.851394	47.131149
2582.535616	135995.202550	47.136154
2578.791058	134656.615171	47.141159
2574.965583	133333.078746	47.146164
2571.556249	132004.593715	47.151169
2567.748453	130680.739911	47.156173
2564.478773	129355.481542	47.161178
2560.691592	128028.462913	47.166183
2557.124170	126710.762513	47.171188
2553.466902	125386.962168	47.176193
2550.069445	124071.672853	47.181197
2546.231284	122748.495717	47.186202
2542.346206	121438.723580	47.191207
2538.454282	120141.967879	47.196212
2535.003582	118824.178284	47.201217
2531.494218	117527.654243	47.206221
2527.593691	116230.447456	47.211226
2524.132537	114933.623888	47.216231
2520.579456	113645.290371	47.221236
2516.814781	112352.992186	47.226241
2513.128117	111065.203503	47.231245
2509.643913	109770.500680	47.236250
2506.378562	108493.279199	47.241255
2502.347856	107218.919339	47.246260
2498.881010	105924.661724	47.251265
2495.275597	104658.529931	47.256269
2491.333137	103382.011489	47.261274
2488.032559	102111.034232	47.266279
2484.131000	100845.372997	47.271284
2480.717392	99574.155616	47.276289
2476.987445	98310.968301	47.281293
2473.151184	97043.945784	47.286298
2469.778343	95791.338102	47.291303
2465.967181	94528.631796	47.296308
2462.287854	93281.891151	47.301313
2458.796044	92034.612519	47.306317
2454.932281	90772.805362	47.311322
2452.239988	89526.305152	47.316327
2448.026600	88296.052563	47.321332
2444.666127	87037.144615	47.326337
2440.751458	85798.576905	47.331341
2437.235659	84561.701733	47.336346
2433.766754	83325.202473	47.341351
2429.485826	82090.230114	47.346356
2425.970925	80855.534631	47.351361
2421.826469	79639.116773	47.356365
2418.715827	78416.201698	47.361370
2415.332304	77193.853283	47.366375
2411.112872	75984.580358	47.371380
2407.806500	74766.786100	47.376385
2404.219002	73561.332248	47.381389
2400.460208	72359.514941	47.386394
2396.732636	71153.468106	47.391399
2393.196335	69955.267857	47.396404
2389.905959	68754.760648	47.401409
2385.886036	67564.865370	47.406413
2382.263840	66380.015564	47.411418
2378.865407	65186.058354	47.416423
2375.012240	63999.686215	47.421428
2371.284780	62811.516180	47.426433
2367.990142	61637.792007	47.431437
2364.226702	60451.333270	47.436442
2360.496757	59273.842300	47.441447
2357.048988	58105.038185	47.446452
2353.612703	56930.305121	47.451457
2349.747218	55774.134608	47.456461
2346.095029	54604.618695	47.461466
2342.522108	53441.263803	47.466471
2338.689687	52285.315072	47.471476
2335.345521	51120.250293	47.476481
2331.708402	49979.279955	47.481485
2327.825950	48812.220580	47.486490
2323.893115	47676.415183	47.491495
2320.343628	46535.602290	47.496500
2317.109608	45393.896919	47.501505
2313.378623	44251.889619	47.506509
2309.545511	43122.975418	47.511514
2305.979978	41987.634210	47.516519
2301.998597	40862.992731	47.521524
2298.016805	39741.965909	47.526529
2294.472252	38629.677592	47.531533
2290.863991	37522.902144	47.536538
2287.132807	36411.524286	47.541543
2283.509836	35316.757533	47.546548
2279.897627	34210.153873	47.551553
2275.937543	33121.251624	47.556557
2272.251860	32037.724828	47.561562
2268.326056	30946.420196	47.566567
2264.434989	29876.283735	47.571572
2260.611253	28795.444357	47.576577
2256.849922	27723.700931	47.581581
2253.316411	26669.929182	47.586586
2249.494617	25636.798842	47.591591
2245.548596	24587.463999	47.596596
2241.934842	23555.769841	47.601601
2237.678315	22527.631380	47.606605
2234.131611	21495.893776	47.611610
2229.957603	20485.718626	47.616615
2225.587812	19501.260293	47.621620
2221.740062	18510.518175	47.626625
2217.378430	17538.723693	47.631629
2213.043014	16581.353330	47.636634
2208.532059	15644.301029	47.641639
2203.176465	14745.368419	47.646644
2197.826225	13867.199735	47.651649
2192.693590	13020.070834	47.656653
2187.723823	12200.073250	47.661658
2182.854028	11402.328677	47.666663
2177.821477	10638.800455	47.671668
2173.103562	9884.326392	47.676673
2167.883447	9177.239425	47.681677
2163.312486	8486.663704	47.686682
2158.872208	7820.863665	47.691687
2154.272258	7186.126774	47.696692
2149.866927	6570.684201	47.701697
2145.383978	5973.152491	47.706701
2141.375262	5411.748446	47.711706
2137.456385	4849.031071	47.716711
2133.341265	4314.383790	47.721716
2129.301887	3789.749529	47.726721
2125.441056	3290.499696	47.731725
2121.157218	2799.753124	47.736730
2116.994125	2325.885151	47.741735
2112.843104	1875.625747	47.746740
2107.921932	1447.155997	47.751745
2102.123859	1086.738963	47.756749
2096.134982	738.998908	47.761754
2090.628333	444.153277	47.766759
2083.821526	208.834471	47.771764
2071.570215	166.416701	47.776769
2060.379848	170.825216	47.781773
2053.977180	180.207965	47.786778
2051.287709	176.367082	47.791783
2049.310207	177.866062	47.796788
2048.657575	184.444487	47.801793
2047.475530	179.899491	47.806797
2045.440058	174.203521	47.811802
2043.545695	175.104187	47.816807
2040.264785	184.637573	47.821812
2037.560514	184.383619	47.826817
2034.351122	182.914699	47.831821
2030.958534	181.803483	47.836826
2027.991545	177.272023	47.841831
2024.737811	177.898167	47.846836
2021.298432	176.022304	47.851841
2017.916524	180.344866	47.856845
2014.578113	182.069454	47.861850
2011.285117	172.599666	47.866855
2008.078217	173.873398	47.871860
2005.109980	168.171530	47.876865
2001.728091	179.033707	47.881869
1998.596373	174.161030	47.886874
1995.277691	170.760313	47.891879
1991.801713	184.279007	47.896884
1988.593998	180.436974	47.901889
1985.233043	175.467291	47.906893
1981.417335	185.527308	47.911898
1978.376987	173.553383	47.916903
1975.201301	168.298446	47.921908
1971.787774	183.341823	47.926913
1968.237134	177.572906	47.931917
1964.554759	176.114744	47.936922
1961.527362	171.143497	47.941927
1957.699223	179.281862	47.946932
1954.650803	169.457446	47.951937
1951.609399	175.074529	47.956941
1947.657897	177.527836	47.961946
1944.379499	163.892211	47.966951
1940.522487	170.348781	47.971956
1937.590853	170.285457	47.976961
1934.190036	177.996286	47.981965
1930.135582	176.172407	47.986970
1926.782550	163.734900	47.991975
1923.760580	180.555190	47.996980
1920.083473	171.439780	48.001985
1916.461491	176.198577	48.006989
1913.189002	176.792888	48.011994
1909.864301	173.908843	48.016999
1906.027381	174.300408	48.022004
1903.358406	174.347856	48.027009
1899.613118	183.523661	48.032013
1896.029645	176.779126	48.037018
1892.937273	173.305063	48.042023
1888.920853	174.787766	48.047028
1885.432421	171.853419	48.052033
1882.180114	174.966142	48.057037
1878.881876	174.580546	48.062042
1875.392726	173.854659	48.067047
1871.990848	168.021373	48.072052
1868.529887	173.780063	48.077057
1865.200323	163.487140	48.082061
1861.342515	175.784262	48.087066
1857.642789	176.989624	48.092071
1854.618352	172.685513	48.097076
1850.884391	176.952480	48.102081
1847.303527	174.026283	48.107085
1843.928625	167.426308	48.112090
1840.818248	163.088196	48.117095
1837.136876	168.916187	48.122100
1833.571553	156.113306	48.127105
1830.460991	165.847867	48.132109
1826.479324	162.873668	48.137114
1823.152401	161.182760	48.142119
1819.450316	171.066843	48.147124
1816.548558	158.732775	48.152129
1813.054512	167.318777	48.157133
1809.202940	165.206930	48.162138
1805.848788	167.149182	48.167143
1802.411613	166.415186	48.172148
1798.763119	162.695985	48.177153
1795.217492	158.033691	48.182157
1791.656164	162.444503	48.187162
1788.789643	160.298736	48.192167
1784.913642	165.211220	48.197172
1781.438388	162.325471	48.202177
1777.882137	158.354558	48.207181
1774.107652	165.285489	48.212186
1771.392228	162.780716	48.217191
1767.636422	165.402779	48.222196
1764.084480	154.154432	48.227201
1760.318037	160.619028	48.232205
1756.710700	155.944260	48.237210
1753.677304	155.691267	48.242215
1750.130806	162.099298	48.247220
1746.545046	163.407086	48.252225
1743.149128	166.751134	48.257229
1739.656824	168.300567	48.262234
1736.097508	166.728316	48.267239
1732.269389	161.600882	48.272244
1729.255098	153.644194	48.277249
1725.658664	155.880655	48.282253
1722.093051	163.503425	48.287258
1718.834956	155.727267	48.292263
1714.953881	154.436338	48.297268
1711.686944	150.761865	48.302273
1708.212641	161.834717	48.307277
1704.734775	154.687756	48.312282
1701.028874	155.318323	48.317287
1697.219103	165.301548	48.322292
1693.743173	155.518834	48.327297
1690.893511	154.759369	48.332301
1686.906747	152.289073	48.337306
1683.768983	153.539424	48.342311
1680.722583	153.835825	48.347316
1676.927215	158.207369	48.352321
1673.221933	157.743171	48.357325
1669.633229	164.179979	48.362330
1666.337193	151.970957	48.367335
1662.353813	165.695672	48.372340
1659.247359	153.839802	48.377345
1656.454932	154.776681	48.382349
1652.285433	162.288336	48.387354
1648.817027	156.677526	48.392359
1645.125840	159.245224	48.397364
1641.461214	149.381335	48.402369
1638.445934	150.827668	48.407373
1634.662973	157.839060	48.412378
1631.493219	151.330453	48.417383
1628.008766	153.929077	48.422388
1624.204614	156.255030	48.427393
1620.827996	155.685628	48.432397
1617.583194	156.047902	48.437402
1614.129984	148.403567	48.442407
1610.070032	149.064269	48.447412
1606.628684	145.989780	48.452417
1603.537111	146.619146	48.457421
1599.755619	153.712577	48.462426
1596.271705	139.925787	48.467431
1592.628422	151.246575	48.472436
1589.049580	144.672298	48.477441
1586.022169	142.165790	48.482445
1582.012116	146.805085	48.487450
1579.114822	143.066478	48.492455
1575.456848	139.095748	48.497460
1571.830450	143.270032	48.502465
1568.229640	144.270182	48.507469
1564.799231	152.646962	48.512474
1561.506247	147.217544	48.517479
1557.526655	143.651504	48.522484
1554.560532	138.537934	48.527489
1550.877350	145.328084	48.532493
1546.967714	140.697554	48.537498
1544.126751	140.870092	48.542503
1539.841196	147.472950	48.547508
1536.529098	149.598530	48.552513
1533.073349	144.609057	48.557517
1529.812527	149.191214	48.562522
1526.962309	132.992537	48.567527
1523.146896	139.623054	48.572532
1519.650238	147.485022	48.577537
1516.483242	139.906665	48.582541
1512.350973	143.789982	48.587546
1509.183586	143.257473	48.592551
1505.086899	142.240825	48.597556
1501.541747	148.547472	48.602561
1498.735033	144.870643	48.607565
1494.674282	143.111209	48.612570
1491.272164	143.950570	48.617575
1487.575713	142.061350	48.622580
1484.299780	139.093895	48.627585
1481.135848	142.442836	48.632589
1477.345318	154.916180	48.637594
1473.843052	147.548504	48.642599
1469.841618	154.461264	48.647604
1467.000409	153.836584	48.652609
1463.559845	148.003189	48.657613
1459.664505	147.461251	48.662618
1456.016817	138.860320	48.667623
1452.853139	150.343358	48.672628
1449.355961	140.975377	48.677633
1446.075157	143.814268	48.682637
1442.358397	152.296015	48.687642
1438.966998	148.539878	48.692647
1435.243041	157.022755	48.697652
1431.742482	152.008696	48.702657
1428.633767	146.990252	48.707661
1424.681428	142.834701	48.712666
1421.540771	144.594954	48.717671
1417.803461	145.515281	48.722676
1414.142673	144.370327	48.727681
1411.221390	144.707336	48.732685
1406.924702	144.282027	48.737690
1404.016962	149.631539	48.742695
1400.437181	150.729698	48.747700
1396.927165	140.841723	48.752705
1393.533622	140.743290	48.757709
1389.586758	137.785977	48.762714
1386.263935	134.816406	48.767719
1382.866998	144.016906	48.772724
1379.445797	138.088767	48.777729
1376.175491	142.881262	48.782733
1372.243883	148.868785	48.787738
1368.375317	150.432945	48.792743
1365.220950	139.568648	48.797748
1362.030879	133.860605	48.802753
1358.392774	141.074032	48.807757
1354.485569	137.294267	48.812762
1351.385511	132.850311	48.817767
1348.055993	134.190890	48.822772
1344.451487	130.718092	48.827777
1340.823311	128.615760	48.832781
1337.507426	137.503021	48.837786
1333.780176	138.649597	48.842791
1330.526661	138.478646	48.847796
1326.543251	145.600604	48.852801
1323.611520	141.370755	48.857805
1319.423137	144.313791	48.862810
1316.308597	135.022016	48.867815
1312.696753	142.623658	48.872820
1309.416991	142.216373	48.877825
1306.063071	143.351976	48.882829
1302.266284	147.761831	48.887834
1298.651251	138.124461	48.892839
1295.654401	141.760516	48.897844
1291.924468	145.944771	48.902849
1288.503715	145.227366	48.907853
1284.868582	156.043920	48.912858
1281.325238	147.072382	48.917863
1277.756174	144.878560	48.922868
1273.997798	145.027109	48.927873
1270.514635	142.693290	48.932877
1267.027002	148.130451	48.937882
1264.134353	132.498521	48.942887
1260.551668	142.655122	48.947892
1256.742439	142.232663	48.952897
1253.386908	135.857691	48.957901
1249.868298	147.000861	48.962906
1246.290876	129.052675	48.967911
1243.147930	143.534946	48.972916
1239.647488	142.814215	48.977921
1235.928168	140.340208	48.982925
1232.105850	147.225007	48.987930
1228.660658	136.713184	48.992935
1225.319334	143.769460	48.997940
1221.411263	142.160248	49.002945
1218.399295	131.836879	49.007949
1214.682264	137.199233	49.012954
1211.123188	140.648078	49.017959
1207.512944	134.192776	49.022964
1204.356322	138.492954	49.027969
1200.952180	137.674903	49.032973
1197.186076	143.244266	49.037978
1193.913438	134.088023	49.042983
1190.227179	145.108755	49.047988
1186.659141	142.383291	49.052993
1183.515716	140.749301	49.057997
1179.555296	138.284587	49.063002
1176.687280	132.311057	49.068007
1172.965322	138.743558	49.073012
1169.157249	136.758041	49.078017
1165.536297	133.863698	49.083021
1161.796471	141.583499	49.088026
1158.679681	132.225701	49.093031
1155.259283	128.458398	49.098036
1151.799408	140.924349	49.103041
1148.352015	135.864119	49.108045
1144.530549	135.348707	49.113050
1141.304956	132.816425	49.118055
1137.913818	133.961074	49.123060
1134.216973	143.686325	49.128065
1130.901506	133.166894	49.133069
1127.143075	135.495358	49.138074
1123.753091	131.802399	49.143079
1120.100531	138.689129	49.148084
1116.606272	141.096462	49.153089
1113.258172	131.021916	49.158093
1109.434679	143.218937	49.163098
1105.940600	137.466835	49.168103
1102.672799	137.981575	49.173108
1099.086892	139.270627	49.178113
1095.673807	128.516558	49.183117
1092.297523	148.834617	49.188122
1088.475164	130.741360	49.193127
1085.509783	134.090968	49.198132
1081.357952	139.284157	49.203137
1077.979524	141.572128	49.208141
1074.908083	143.524132	49.213146
1071.361024	134.372940	49.218151
1067.937692	142.913261	49.223156
1064.009389	142.756297	49.228161
1060.707708	135.828800	49.233165
1056.931034	136.853503	49.238170
1053.743968	139.260219	49.243175
1049.940234	142.614544	49.248180
1046.823439	142.792445	49.253185
1043.174918	126.351972	49.258189
1039.610901	133.753215	49.263194
1036.267636	134.668938	49.268199
1032.707023	135.507960	49.273204
1028.961728	138.498799	49.278209
1025.554631	129.578820	49.283213
1021.730327	140.526297	49.288218
1018.898280	138.562034	49.293223
1015.526963	133.050180	49.298228
1011.536287	131.109139	49.303233
1008.712453	132.579464	49.308237
1004.476086	143.388984	49.313242
1001.000883	137.551711	49.318247
997.377372	131.914835	49.323252
993.945014	137.400372	49.328257
990.612243	136.713593	49.333261
987.242820	138.911598	49.338266
983.710215	123.554007	49.343271
980.123945	131.582016	49.348276
976.227694	133.792909	49.353281
973.345655	136.787810	49.358285
969.688996	149.221349	49.363290
966.397377	134.126584	49.368295
962.874862	137.604590	49.373300
959.056123	141.771227	49.378305
955.672602	131.531451	49.383309
952.219180	134.150748	49.388314
948.286253	134.064160	49.393319
944.985649	136.146998	49.398324
941.551722	142.499675	49.403329
938.174697	129.541201	49.408333
934.507124	139.091082	49.413338
931.061869	133.638296	49.418343
927.496001	134.152310	49.423348
923.683181	134.508838	49.428353
920.643674	130.248547	49.433357
916.787244	138.989603	49.438362
913.746728	136.099389	49.443367
910.323433	134.740272	49.448372
906.623818	135.895337	49.453377
903.108334	135.392224	49.458381
899.334522	137.555502	49.463386
895.667081	126.357294	49.468391
892.381892	125.372032	49.473396
889.191302	137.754753	49.478401
885.645796	136.664720	49.483405
882.134977	136.603813	49.488410
878.686300	134.881684	49.493415
875.047189	139.570723	49.498420
871.551862	136.410052	49.503425
868.325719	133.536266	49.508429
864.268425	136.892399	49.513434
860.963990	135.476723	49.518439
857.540383	131.630943	49.523444
853.855267	134.561803	49.528449
850.060354	127.736940	49.533453
846.323408	130.824615	49.538458
843.604232	134.183195	49.543463
840.312921	131.278495	49.548468
836.429954	140.795696	49.553473
833.345676	132.511790	49.558477
829.370192	135.472309	49.563482
826.086673	137.011505	49.568487
822.226658	131.908453	49.573492
819.046270	131.308606	49.578497
815.864411	132.249751	49.583501
812.105509	134.572079	49.588506
808.526970	128.206902	49.593511
804.978333	129.623104	49.598516
800.819064	137.389720	49.603521
797.373946	128.820647	49.608525
794.194140	128.720595	49.613530
791.642832	129.455439	49.618535
787.789226	127.281059	49.623540
783.949244	134.311141	49.628545
781.222208	126.974235	49.633549
776.837780	139.072529	49.638554
773.132966	127.715716	49.643559
770.048050	131.716887	49.648564
766.305253	132.578210	49.653569
763.113807	129.271920	49.658573
759.135772	139.316566	49.663578
755.612475	126.200751	49.668583
752.533667	130.991914	49.673588
749.023541	138.805593	49.678593
745.909502	129.219744	49.683597
741.825466	136.775282	49.688602
738.362008	122.074547	49.693607
734.677473	136.255748	49.698612
731.278969	132.561113	49.703617
727.902431	131.435190	49.708621
724.210172	139.125537	49.713626
720.909242	122.311265	49.718631
717.460511	126.353606	49.723636
713.774981	136.222743	49.728641
710.491901	125.075168	49.733645
706.513074	130.032600	49.738650
702.763336	122.938140	49.743655
700.065266	123.056910	49.748660
696.510593	126.726705	49.753665
693.143746	122.878432	49.758669
689.327885	133.679153	49.763674
685.585298	130.332653	49.768679
682.530861	124.435953	49.773684
678.599198	129.591656	49.778689
675.737625	128.913456	49.783693
671.897362	130.802488	49.788698
668.420161	125.889495	49.793703
664.648234	127.710880	49.798708
660.831466	130.273284	49.803713
657.695110	123.266283	49.808717
654.453739	129.974870	49.813722
650.848018	121.054530	49.818727
647.436054	121.218678	49.823732
643.850777	122.542601	49.828737
640.376428	123.871299	49.833741
636.618522	135.438086	49.838746
633.385585	122.327482	49.843751
629.896994	124.395573	49.848756
626.380352	127.315950	49.853761
622.739139	132.682453	49.858765
618.977624	122.742480	49.863770
615.656116	117.811456	49.868775
612.493964	112.773220	49.873780
608.904033	129.410540	49.878785
605.465953	121.466881	49.883789
601.662899	135.397760	49.888794
598.110914	138.130694	49.893799
594.826067	129.046226	49.898804
591.343976	131.296813	49.903809
588.137558	125.237289	49.908813
584.156995	122.984805	49.913818
580.780882	129.100745	49.918823
577.509062	121.156371	49.923828
573.190374	130.412865	49.928833
570.591862	122.103612	49.933837
566.805902	129.169602	49.938842
563.134851	117.263445	49.943847
559.720232	123.021587	49.948852
556.013311	120.903430	49.953857
552.579875	111.551196	49.958861
548.740837	121.634246	49.963866
545.719218	117.254235	49.968871
542.568497	124.666832	49.973876
538.847204	124.272024	49.978881
535.264295	123.140532	49.983885
531.431683	120.839590	49.988890
528.340522	122.219046	49.993895
524.764959	130.808673	49.998900
521.188547	129.214258	50.003905
518.026286	124.679112	50.008909
514.065190	135.486819	50.013914
510.790191	132.930869	50.018919
506.967837	120.520087	50.023924
503.493269	128.030875	50.028929
500.309846	118.563571	50.033933
496.489226	132.696548	50.038938
493.076914	129.532522	50.043943
489.641974	124.774339	50.048948
485.870358	131.613484	50.053953
482.907145	127.553378	50.058957
479.209671	131.780295	50.063962
476.046996	127.941258	50.068967
472.075644	125.159034	50.073972
468.436568	127.310867	50.078977
464.576085	126.991675	50.083981
461.340224	132.326382	50.088986
457.938808	121.475871	50.093991
454.702735	118.879047	50.098996
451.247209	123.631227	50.104001
448.099601	115.873100	50.109005
444.102931	118.988953	50.114010
440.510359	124.389028	50.119015
437.114214	120.668835	50.124020
433.545283	126.862480	50.129025
430.292414	120.506576	50.134029
426.441325	127.579653	50.139034
423.229038	123.704116	50.144039
420.039209	128.620336	50.149044
416.312704	139.283766	50.154049
412.894779	129.163524	50.159053
409.053743	135.475732	50.164058
405.531522	120.246531	50.169063
401.841863	126.807111	50.174068
398.416583	126.764630	50.179073
395.057589	123.326538	50.184077
391.538358	124.494679	50.189082
387.808294	126.224195	50.194087
384.518778	124.179936	50.199092
380.835465	116.277958	50.204097
377.491934	127.112360	50.209101
373.974589	126.220601	50.214106
370.519708	120.994193	50.219111
366.974762	120.258621	50.224116
363.301036	132.650704	50.229121
360.119576	119.165171	50.234125
356.567336	124.182471	50.239130
353.096703	115.291735	50.244135
349.755206	113.160721	50.249140
346.008120	117.544153	50.254145
342.693123	121.382176	50.259149
339.090673	118.377713	50.264154
335.837256	114.590914	50.269159
332.285458	126.264711	50.274164
328.028003	127.491568	50.279169
324.736675	123.824605	50.284173
321.061713	123.368847	50.289178
317.780718	123.705593	50.294183
314.852679	118.744696	50.299188
311.100179	119.886133	50.304193
307.576606	117.805803	50.309197
304.089347	119.294837	50.314202
300.332638	125.204730	50.319207
297.307393	115.276140	50.324212
293.182362	122.958490	50.329217
289.678221	122.308307	50.334221
286.149770	115.343901	50.339226
282.679645	118.478579	50.344231
279.561931	118.362654	50.349236
275.950695	116.656738	50.354241
272.332559	117.318398	50.359245
268.924356	120.294684	50.364250
265.398282	124.763750	50.369255
262.303211	120.626306	50.374260
258.401890	112.552897	50.379265
255.106025	120.133844	50.384269
251.494939	116.479038	50.389274
248.227612	122.489457	50.394279
244.322027	121.373832	50.399284
240.742587	122.950097	50.404289
237.330942	115.296698	50.409293
233.901936	127.707428	50.414298
230.400676	123.462784	50.419303
226.888635	121.415482	50.424308
223.126060	126.870741	50.429313
219.878074	120.223096	50.434317
216.372945	127.011099	50.439322
213.125105	116.019591	50.444327
209.706363	119.475278	50.449332
205.995470	122.470532	50.454337
202.579536	117.994235	50.459341
199.086750	116.364708	50.464346
195.052304	116.066561	50.469351
191.959783	116.383319	50.474356
188.435598	125.474370	50.479361
184.920661	109.987890	50.484365
181.112534	109.050016	50.489370
177.622715	114.690350	50.494375
173.910880	116.319021	50.499380
170.395080	117.439254	50.504385
167.414010	114.271081	50.509389
164.454113	119.597447	50.514394
160.506369	123.999734	50.519399
157.251348	118.564938	50.524404
153.533606	116.739718	50.529409
149.762850	117.675275	50.534413
146.306417	112.389099	50.539418
142.208667	120.073563	50.544423
139.181800	113.786783	50.549428
135.667468	117.213179	50.554433
132.774300	114.338132	50.559437
129.124039	111.983496	50.564442
125.106907	118.117750	50.569447
121.536596	108.144921	50.574452
118.149724	115.037813	50.579457
114.638891	113.417477	50.584461
111.769078	114.025239	50.589466
107.559769	117.592164	50.594471
104.461347	116.277379	50.599476
100.722723	116.214503	50.604481
97.363017	112.855741	50.609485
93.780263	116.931951	50.614490
89.910680	122.366061	50.619495
86.740984	111.783152	50.624500
83.321592	120.848325	50.629505
79.973093	110.780652	50.634509
76.800285	109.322508	50.639514
72.859027	119.149653	50.644519
69.407008	114.141230	50.649524
65.539214	117.306655	50.654529
62.011814	113.952035	50.659533
58.713253	112.614840	50.664538
55.087007	123.063355	50.669543
51.675579	118.194112	50.674548
48.018013	120.611598	50.679553
44.727123	112.015553	50.684557
41.406554	113.782292	50.689562
37.914771	112.519672	50.694567
34.262540	106.296116	50.699572
29.900701	120.188158	50.704577
27.168848	117.563121	50.709581
23.590689	116.911989	50.714586
20.393792	129.248449	50.719591
16.891997	122.147112	50.724596
13.137187	124.738037	50.729601
9.396326	115.731616	50.734605
6.147341	116.338711	50.739610
2.531290	118.563049	50.744615