Thu Aug 25 12:49:25 2022

Number of Points = 9924

Depth (nm)	Load (N)	Time (s)
2.250134	103.269089	0.000000
2.355250	97.712763	0.005005
2.030467	101.730956	0.010010
1.848199	104.983331	0.015014
2.677767	102.486768	0.020019
2.160284	96.028237	0.025024
1.775357	83.664312	0.030029
1.723184	90.211941	0.035034
1.523445	87.920946	0.040038
1.739166	74.086673	0.045043
1.078153	74.285079	0.050048
0.818327	58.927621	0.055053
0.780128	45.667832	0.060058
0.481293	53.060856	0.065062
0.640100	39.732239	0.070067
-0.016039	31.049181	0.075072
0.050458	17.257315	0.080077
-0.401701	18.334162	0.085082
-1.231137	9.010712	0.090086
-1.172675	2.079160	0.095091
-1.828155	5.797968	0.100096
-2.112300	9.525034	0.105101
-2.488634	9.552285	0.110106
-3.141428	6.623604	0.115110
-2.861043	0.761436	0.120115
-2.958474	9.144781	0.125120
-2.746969	7.159523	0.130125
-3.334052	7.121718	0.135130
-4.217932	14.172956	0.140134
-4.562924	3.792839	0.145139
-4.398757	20.006647	0.150144
-4.307668	4.369627	0.155149
-4.454520	-1.077587	0.160154
-5.204961	1.298845	0.165158
-5.348977	-7.034163	0.170163
-5.919166	10.351393	0.175168
-5.563961	1.785137	0.180173
-5.700530	10.263200	0.185178
-6.720454	9.669953	0.190182
-6.553913	3.996464	0.195187
-7.376959	11.294434	0.200192
-7.562031	9.032790	0.205197
-7.273208	-1.294771	0.210202
-7.725946	7.827616	0.215206
-7.832021	2.016508	0.220211
-8.510468	4.805604	0.225216
-8.879505	3.544060	0.230221
-9.086773	4.550899	0.235226
-9.357302	6.557907	0.240230
-8.947545	-0.166093	0.245235
-9.149093	6.752923	0.250240
-9.101971	7.286468	0.255245
-9.125058	3.436545	0.260250
-10.303319	5.747131	0.265254
-10.367154	2.425614	0.270259
-10.720243	2.047425	0.275264
-10.899876	6.052346	0.280269
-11.331320	-0.618946	0.285274
-11.921397	-2.114776	0.290278
-11.959462	-5.139772	0.295283
-11.859003	14.026310	0.300288
-12.211873	3.150717	0.305293
-12.189001	7.630111	0.310298
-12.533634	6.627336	0.315302
-12.466545	5.566378	0.320307
-13.374651	20.027788	0.325312
-13.404301	8.313771	0.330317
-13.861248	4.465388	0.335322
-14.105081	8.568953	0.340326
-13.890047	3.144131	0.345331
-14.390640	-2.089468	0.350336
-15.049865	8.568060	0.355341
-15.088173	11.171436	0.360346
-15.268344	10.047980	0.365350
-15.406504	1.157229	0.370355
-15.824613	7.461605	0.375360
-15.644844	6.373501	0.380365
-15.817190	4.166812	0.385370
-16.506807	9.216587	0.390374
-16.618439	-9.245536	0.395379
-16.709390	5.255506	0.400384
-17.050972	-1.834826	0.405389
-17.590276	-6.739655	0.410394
-17.791261	2.283173	0.415398
-17.867543	-4.412128	0.420403
-18.329362	3.645493	0.425408
-18.272029	1.744503	0.430413
-18.516669	8.116613	0.435418
-19.557963	9.276277	0.440422
-19.512407	10.151753	0.445427
-19.719284	8.687631	0.450432
-19.311459	8.139599	0.455437
-19.266063	2.481928	0.460442
-20.083403	9.614489	0.465446
-20.454916	-1.001914	0.470451
-20.691945	3.647915	0.475456
-20.901957	-4.396341	0.480461
-21.125510	2.434371	0.485466
-21.308277	4.585817	0.490470
-21.499538	4.878301	0.495475
-22.465078	1.280451	0.500480
-22.582772	12.511194	0.505485
-22.256160	9.666339	0.510490
-22.790800	5.744708	0.515494
-22.750206	4.548696	0.520499
-23.024310	10.529953	0.525504
-23.570685	2.022703	0.530509
-23.915646	3.003660	0.535514
-24.714165	0.376226	0.540518
-24.021701	9.050258	0.545523
-24.225497	2.931757	0.550528
-24.312542	10.054297	0.555533
-24.712934	4.311450	0.560538
-25.445864	13.373337	0.565542
-25.205419	7.220031	0.570547
-25.423797	4.995244	0.575552
-25.458091	7.499914	0.580557
-25.913042	1.215122	0.585562
-26.533993	10.151894	0.590566
-26.380565	-0.600543	0.595571
-26.804208	0.541439	0.600576
-27.492029	9.574110	0.605581
-27.329969	2.547234	0.610586
-27.960632	1.788593	0.615590
-27.998256	-1.682563	0.620595
-27.880257	1.661952	0.625600
-28.723455	4.252236	0.630605
-28.779381	11.683113	0.635610
-29.308996	6.741962	0.640614
-28.979212	0.957475	0.645619
-29.753400	6.254619	0.650624
-29.628953	-2.870264	0.655629
-29.900354	-1.419942	0.660634
-30.097637	1.508900	0.665638
-30.368333	-5.301471	0.670643
-30.783233	4.074414	0.675648
-31.309702	9.130264	0.680653
-31.256040	4.926630	0.685658
-31.210314	12.740213	0.690662
-31.270914	6.817575	0.695667
-31.950229	1.653108	0.700672
-32.455328	14.523270	0.705677
-32.286788	4.379070	0.710682
-32.764654	20.396077	0.715686
-32.913399	1.003287	0.720691
-33.694651	7.396200	0.725696
-34.369041	1.822837	0.730701
-33.829574	-0.131550	0.735706
-33.958781	5.652995	0.740710
-34.071970	5.961720	0.745715
-34.302450	7.184168	0.750720
-34.245899	5.125113	0.755725
-35.019063	4.989916	0.760730
-35.481288	14.370057	0.765734
-35.430469	1.071048	0.770739
-35.731440	3.424513	0.775744
-35.775751	8.831923	0.780749
-35.716247	4.292015	0.785754
-36.419455	7.325439	0.790758
-36.794322	0.056825	0.795763
-37.115415	1.321944	0.800768
-37.018817	1.623109	0.805773
-37.002890	0.924509	0.810778
-37.808480	-0.515404	0.815782
-38.013351	0.256941	0.820787
-38.158014	-0.948008	0.825792
-38.292211	7.112063	0.830797
-38.991959	-1.038956	0.835802
-39.761104	13.742361	0.840806
-39.603936	3.840389	0.845811
-39.483897	12.300390	0.850816
-40.111587	12.958651	0.855821
-39.817994	7.129213	0.860826
-40.395246	13.569258	0.865830
-40.048024	12.919989	0.870835
-40.530950	23.676453	0.875840
-41.235602	11.213984	0.880845
-41.265292	7.940901	0.885850
-41.989409	5.716263	0.890854
-41.511008	8.270315	0.895859
-41.506389	8.342282	0.900864
-42.172086	14.138123	0.905869
-42.822641	1.433066	0.910874
-43.311726	-0.107059	0.915878
-43.171122	7.479683	0.920883
-43.118909	0.384598	0.925888
-43.080455	9.028224	0.930893
-43.029026	5.002110	0.935898
-44.006849	13.551875	0.940902
-43.723690	6.733813	0.945907
-44.385233	-1.331442	0.950912
-44.922930	8.051030	0.955917
-45.370365	4.387821	0.960922
-45.959952	5.549477	0.965926
-45.870355	-1.143339	0.970931
-46.074237	5.592542	0.975936
-46.016781	5.785944	0.980941
-45.887924	7.736702	0.985946
-46.311921	3.889487	0.990950
-46.429031	-4.865351	0.995955
-46.778043	6.012488	1.000960
-47.467476	5.990723	1.005965
-47.602937	2.886075	1.010970
-48.042984	4.375478	1.015974
-47.659640	5.555532	1.020979
-47.665782	6.802940	1.025984
-48.285347	7.754158	1.030989
-48.516253	2.582709	1.035994
-49.089966	7.136596	1.040998
-49.350144	-1.168719	1.046003
-50.097266	12.052575	1.051008
-50.427678	15.296509	1.056013
-50.199253	2.282884	1.061018
-50.443561	8.499917	1.066022
-50.356383	-0.641274	1.071027
-50.371726	3.802976	1.076032
-50.360787	2.156030	1.081037
-50.901435	5.053251	1.086042
-51.357846	6.519908	1.091046
-51.644028	9.968883	1.096051
-52.021564	3.172088	1.101056
-52.693194	8.484802	1.106061
-53.101569	6.191710	1.111066
-53.098277	20.051568	1.116070
-53.045041	11.333307	1.121075
-53.392622	9.948180	1.126080
-53.788515	8.820561	1.131085
-53.042082	9.140127	1.136090
-53.526410	14.198867	1.141094
-53.951972	0.882754	1.146099
-54.511957	8.851353	1.151104
-54.657068	6.210126	1.156109
-54.843292	-0.293940	1.161114
-56.116220	2.816098	1.166118
-55.751801	3.480260	1.171123
-56.001619	4.882908	1.176128
-56.126232	11.147626	1.181133
-56.267492	2.735092	1.186138
-56.479811	-2.543672	1.191142
-56.404607	-0.805972	1.196147
-56.733303	8.021732	1.201152
-57.671106	5.628097	1.206157
-57.818806	7.527275	1.211162
-58.159886	12.860963	1.216166
-57.971093	7.351668	1.221171
-58.055081	10.746814	1.226176
-58.222685	15.835022	1.231181
-58.690586	9.267521	1.236186
-59.762166	17.041037	1.241190
-59.390351	0.755761	1.246195
-59.722049	14.098626	1.251200
-59.567871	4.364803	1.256205
-59.465428	1.305136	1.261210
-60.300078	0.568970	1.266214
-60.449437	1.079516	1.271219
-60.908407	0.857125	1.276224
-61.264134	3.801302	1.281229
-61.004271	4.978557	1.286234
-61.734217	10.063127	1.291238
-61.564225	6.815704	1.296243
-62.073471	-2.703432	1.301248
-62.669731	-0.300535	1.306253
-62.481093	2.843085	1.311258
-62.984639	12.122131	1.316262
-62.413334	3.506197	1.321267
-63.233091	4.915891	1.326272
-63.799407	6.542139	1.331277
-64.040408	-0.886652	1.336282
-64.425061	9.383003	1.341286
-64.413595	7.536656	1.346291
-64.405579	5.308035	1.351296
-64.662008	8.179707	1.356301
-65.071670	1.872003	1.361306
-65.810736	-3.681729	1.366310
-65.562747	5.169507	1.371315
-65.972054	-6.769745	1.376320
-66.282964	2.922039	1.381325
-65.684051	-6.109505	1.386330
-66.254682	7.587168	1.391334
-66.492561	-2.866668	1.396339
-66.916186	6.766848	1.401344
-67.371177	1.402722	1.406349
-67.852621	5.261942	1.411354
-67.821209	9.135717	1.416358
-68.050873	10.519390	1.421363
-68.517157	6.118815	1.426368
-68.867192	13.339509	1.431373
-68.603303	5.587994	1.436378
-68.626627	6.724200	1.441382
-68.874886	1.615582	1.446387
-69.725211	-2.807072	1.451392
-70.086245	-2.279178	1.456397
-70.035476	2.066127	1.461402
-70.145010	4.528801	1.466406
-70.378815	7.776579	1.471411
-71.408116	8.209868	1.476416
-71.554664	-0.951646	1.481421
-71.176751	4.785073	1.486426
-71.892815	13.445684	1.491430
-71.603075	7.088502	1.496435
-71.572163	4.894259	1.501440
-71.917513	4.682540	1.506445
-72.544157	11.810533	1.511450
-73.066434	12.351038	1.516454
-73.059100	7.847778	1.521459
-73.393517	6.546012	1.526464
-73.239178	13.383954	1.531469
-73.571330	3.485890	1.536474
-73.954548	9.208995	1.541478
-74.185956	9.814655	1.546483
-74.463586	7.361872	1.551488
-74.979640	12.169319	1.556493
-75.340507	-0.679198	1.561498
-75.862626	14.550630	1.566502
-75.659329	8.479076	1.571507
-75.884264	4.493103	1.576512
-75.785254	0.573432	1.581517
-75.677959	2.568696	1.586522
-76.520568	4.187617	1.591526
-77.226479	3.073774	1.596531
-77.334283	1.442271	1.601536
-77.451838	1.539708	1.606541
-77.120655	-1.641221	1.611546
-77.498839	4.735993	1.616550
-78.367787	-5.403823	1.621555
-78.955282	7.406476	1.626560
-79.106551	10.910241	1.631565
-78.786404	5.171556	1.636570
-78.890038	10.831871	1.641574
-78.815051	8.061244	1.646579
-78.978916	5.280587	1.651584
-79.875596	7.578698	1.656589
-79.824301	5.083868	1.661594
-80.482783	3.140016	1.666598
-80.471388	5.928593	1.671603
-80.976717	2.593998	1.676608
-81.371401	7.512140	1.681613
-81.410576	7.378997	1.686618
-81.883557	6.374190	1.691622
-81.726055	15.650897	1.696627
-81.615737	10.308922	1.701632
-82.210238	9.528801	1.706637
-82.829543	-0.735555	1.711642
-83.382814	4.678836	1.716646
-83.448858	-1.885187	1.721651
-83.544733	1.752265	1.726656
-83.570667	8.539358	1.731661
-83.332034	-7.623799	1.736666
-83.719449	7.603899	1.741670
-84.301431	4.711587	1.746675
-84.537444	8.342526	1.751680
-84.565143	7.097104	1.756685
-84.480317	-3.363003	1.761690
-85.929402	9.221632	1.766694
-85.971467	6.947075	1.771699
-85.972493	-0.323164	1.776704
-86.288995	4.557416	1.781709
-85.820399	5.945573	1.786714
-86.434048	9.015587	1.791718
-86.581340	0.721061	1.796723
-87.240902	2.909252	1.801728
-87.617145	5.230219	1.806733
-87.308228	5.649975	1.811738
-87.779154	8.915925	1.816742
-88.013160	1.903655	1.821747
-88.597416	2.083713	1.826752
-88.967984	2.053117	1.831757
-89.199922	8.679499	1.836762
-89.444755	17.756657	1.841766
-89.428914	-4.189753	1.846771
-89.280307	0.168693	1.851776
-89.668252	11.555672	1.856781
-90.171389	3.029001	1.861786
-90.672558	12.408914	1.866790
-90.808394	-0.376785	1.871795
-90.931140	0.056825	1.876800
-91.002846	7.176956	1.881805
-91.033853	9.554561	1.886810
-91.634117	10.509085	1.891814
-92.126159	9.779349	1.896819
-92.262591	6.538812	1.901824
-92.300440	4.399636	1.906829
-92.368512	8.750907	1.911834
-92.570991	9.352035	1.916838
-93.090779	-1.184176	1.921843
-93.663088	8.535913	1.926848
-93.953208	1.358430	1.931853
-93.729920	10.292630	1.936858
-94.058519	11.343792	1.941862
-94.315817	2.971590	1.946867
-95.202533	-3.381581	1.951872
-95.415464	-3.708961	1.956877
-95.122722	-6.719350	1.961882
-95.359525	3.868820	1.966886
-95.255922	-2.617381	1.971891
-95.479782	0.072015	1.976896
-95.904894	1.030732	1.981901
-96.448575	-6.451867	1.986906
-96.750173	-2.225358	1.991910
-96.806197	3.724886	1.996915
-96.806723	0.882439	2.006912
-96.896859	5.138111	2.016909
-97.040194	-7.691391	2.026906
-96.335671	9.310581	2.036902
-95.378221	7.326239	2.046899
-94.662733	4.340770	2.056896
-94.547536	10.401600	2.066893
-93.647321	1.776989	2.076890
-93.230729	-1.107792	2.086886
-92.974800	4.547679	2.096883
-92.584005	10.812414	2.106880
-91.872892	7.808623	2.116877
-91.697762	3.558335	2.126874
-90.626016	6.067050	2.136870
-90.381221	8.055941	2.146867
-90.107754	3.299234	2.156864
-89.108625	6.560596	2.166861
-88.718903	2.552283	2.176858
-88.432283	6.869298	2.186854
-87.877710	0.962977	2.196851
-86.967866	10.019588	2.206848
-86.813733	3.821217	2.216845
-86.948213	4.567566	2.226842
-86.080952	0.392561	2.236838
-85.549547	13.395377	2.246835
-84.721021	12.093311	2.256832
-84.441847	6.873208	2.266829
-83.839585	6.807197	2.276826
-83.216973	-0.294547	2.286822
-83.169063	5.070404	2.296819
-82.463669	-2.075988	2.306816
-82.059772	-0.317935	2.316813
-81.199220	0.608289	2.326810
-80.223421	2.384435	2.336806
-80.484399	0.768410	2.346803
-80.118010	-1.348229	2.356800
-79.207192	2.832965	2.366797
-79.177508	6.274742	2.376794
-78.440958	-0.122593	2.386790
-77.464974	-1.260862	2.396787
-77.289979	-1.354958	2.406784
-77.193532	-1.512774	2.416781
-76.156183	1.131212	2.426778
-75.800696	4.968600	2.436774
-75.684559	-4.334606	2.446771
-74.989917	3.859233	2.456768
-74.601335	-1.884861	2.466765
-73.651279	1.488729	2.476762
-73.334276	4.689082	2.486758
-72.992385	6.998547	2.496755
-72.334311	9.660782	2.506752
-72.070184	6.483109	2.516749
-71.303585	12.299321	2.526746
-70.753193	10.996488	2.536742
-70.693902	10.974374	2.546739
-69.941949	9.215471	2.556736
-69.268049	7.262891	2.566733
-68.668539	2.290369	2.576730
-68.506094	4.583603	2.586726
-67.704907	8.579238	2.596723
-66.988818	11.460467	2.606720
-67.018479	15.884064	2.616717
-66.564465	7.098116	2.626714
-65.569036	9.431892	2.636710
-65.112883	1.735339	2.646707
-65.255364	2.156657	2.656704
-64.311928	0.424772	2.666701
-63.614527	8.972978	2.676698
-63.414124	3.115817	2.686694
-62.602392	4.075035	2.696691
-62.338805	1.359948	2.706688
-61.944660	2.980146	2.716685
-61.308651	8.896016	2.726682
-60.917210	2.635119	2.736678
-60.441622	4.765245	2.746675
-59.569830	10.422424	2.756672
-59.471600	10.577943	2.766669
-58.478802	7.526849	2.776666
-57.723183	-1.895567	2.786662
-58.296394	4.637428	2.796659
-57.634995	4.182015	2.806656
-56.581682	8.131811	2.816653
-55.988954	2.865746	2.826650
-56.295405	10.218589	2.836646
-55.268549	8.774577	2.846643
-55.044846	9.296908	2.856640
-54.051895	7.699817	2.866637
-53.540098	12.925562	2.876634
-53.271020	6.329041	2.886630
-52.989722	8.315381	2.896627
-52.359980	6.239841	2.906624
-52.094054	-1.769028	2.916621
-51.109158	3.769058	2.926618
-50.748581	2.454786	2.936614
-50.430170	1.413218	2.946611
-49.363607	2.316669	2.956608
-49.203398	2.896467	2.966605
-49.170122	4.310281	2.976602
-48.231928	-3.721560	2.986598
-47.859860	2.013919	2.996595
-47.141089	1.609706	3.006592
-46.083217	-0.868705	3.016589
-46.138285	2.253732	3.026586
-46.169150	3.931022	3.036582
-45.766676	1.612324	3.046579
-45.075839	3.911465	3.056576
-43.758294	-6.235725	3.066573
-43.246836	-4.995038	3.076570
-43.399998	0.030784	3.086566
-43.397782	-3.767923	3.096563
-42.361772	2.563612	3.106560
-41.731784	-2.508717	3.116557
-41.267590	2.347515	3.126554
-40.715813	2.951491	3.136550
-40.256991	-1.172186	3.146547
-39.568005	1.010036	3.156544
-39.198847	1.661633	3.166541
-38.976723	1.734382	3.176538
-37.958720	-3.693349	3.186534
-37.844822	-0.540367	3.196531
-37.468045	-0.536199	3.206528
-36.600240	-1.489619	3.216525
-35.924387	-0.037104	3.226522
-35.810369	8.025972	3.236518
-35.482094	3.605968	3.246515
-34.431489	3.137091	3.256512
-34.277580	4.332432	3.266509
-33.955612	-1.407561	3.276506
-33.339758	4.045801	3.286502
-32.620845	2.824271	3.296499
-31.880640	3.629973	3.306496
-31.342668	3.162223	3.316493
-31.224519	-0.033758	3.326490
-31.227476	1.151316	3.336486
-30.147272	-4.853200	3.346483
-29.890065	0.992144	3.356480
-29.404161	6.019206	3.366477
-28.874474	4.979380	3.376474
-28.423868	7.693134	3.386470
-27.540915	4.190417	3.396467
-27.439004	10.528933	3.406464
-26.621289	6.048080	3.416461
-26.359756	1.964819	3.426458
-25.746676	2.932992	3.436454
-24.806465	4.394773	3.446451
-24.740665	6.395874	3.456448
-24.407934	-3.039476	3.466445
-23.683124	2.457002	3.476442
-23.036241	5.966802	3.486438
-22.742280	1.590189	3.496435
-22.392843	4.433836	3.506432
-22.013015	0.110293	3.516429
-21.109428	4.083553	3.526426
-20.124074	9.026025	3.536422
-19.876483	7.108566	3.546419
-19.854369	10.481840	3.556416
-19.877382	12.104047	3.566413
-18.912445	12.212466	3.576410
-17.738416	10.216372	3.586406
-17.359200	12.497819	3.596403
-17.265468	3.676454	3.606400
-16.922814	-0.698284	3.616397
-16.198577	4.285101	3.626394
-15.626404	9.710464	3.636390
-15.387249	6.660248	3.646387
-14.726065	7.361125	3.656384
-14.217048	11.925235	3.666381
-13.781392	8.362723	3.676378
-12.833236	8.635330	3.686374
-12.597632	7.761960	3.696371
-12.677128	9.963224	3.706368
-11.456630	6.258733	3.716365
-11.050895	15.365836	3.726362
-10.930302	12.239161	3.736358
-9.963591	9.534282	3.746355
-9.540170	4.722401	3.756352
-9.469054	10.042539	3.766349
-8.499278	1.435542	3.776346
-7.899366	10.410848	3.786342
-7.944421	1.851984	3.796339
-6.856366	6.572458	3.806336
-6.689624	8.313821	3.816333
-6.486059	11.478100	3.826330
-5.800543	7.116164	3.836326
-5.382949	15.480140	3.846323
-4.555446	14.133891	3.856320
-4.189149	16.997074	3.866317
-3.778669	19.004360	3.876314
-3.512054	25.624355	3.886310
-3.262608	27.330587	3.896307
-2.660867	45.121667	3.906304
-2.172667	54.063814	3.916301
-1.381851	67.992226	3.926298
-0.847859	81.016876	3.936294
-0.684304	88.498853	3.946291
-0.446393	111.998415	3.956288
0.000000	119.753670	3.961293
-0.078487	138.229746	3.966298
0.367517	137.242290	3.971302
0.328924	158.189382	3.976307
0.520069	161.373769	3.981312
0.776123	168.410978	3.986317
1.090914	172.794054	3.991322
1.125534	168.131450	3.996326
1.307618	168.659672	4.001331
1.013418	175.349659	4.006336
1.147044	172.968455	4.011341
1.069767	170.601314	4.016346
1.151251	166.038937	4.021350
1.349017	169.263417	4.026355
1.248734	174.135477	4.031360
1.338034	178.148919	4.036365
1.166456	187.869596	4.041370
1.151523	174.349799	4.046374
1.037950	181.166512	4.051379
0.983940	187.107016	4.056384
1.240436	183.406239	4.061389
1.014031	187.532425	4.066394
1.508732	177.628090	4.071398
1.163656	178.745116	4.076403
1.141714	173.673751	4.081408
0.921827	173.334800	4.086413
1.240457	189.534053	4.091418
1.741434	191.926408	4.096422
1.738117	187.949959	4.101427
1.264881	182.329198	4.106432
1.297530	176.682960	4.111437
1.301013	187.382294	4.116442
1.228819	188.345832	4.121446
1.566075	200.283707	4.126451
1.806145	200.518103	4.131456
1.863155	184.066841	4.136461
1.460206	189.536827	4.141466
1.349993	180.635278	4.146470
1.641451	175.562267	4.151475
1.236120	183.440272	4.156480
1.346320	184.640991	4.161485
1.399764	192.886886	4.166490
1.858154	192.198048	4.171494
1.486217	194.980278	4.176499
1.577089	184.924073	4.181504
1.651091	189.113923	4.186509
1.455460	188.030842	4.191514
1.775265	193.314820	4.196518
1.695862	200.983577	4.201523
1.492516	198.193253	4.206528
1.973554	190.338029	4.211533
1.475121	190.124979	4.216538
1.633363	187.996184	4.221542
1.721597	205.924182	4.226547
1.671508	205.305522	4.231552
1.967463	205.376135	4.236557
1.523827	202.677245	4.241562
1.551626	199.448902	4.246566
1.653998	207.092344	4.251571
1.991101	206.485785	4.256576
1.825421	205.480269	4.261581
1.368531	208.725071	4.266586
1.619726	206.202054	4.271590
1.688329	201.910609	4.276595
1.581709	208.960364	4.281600
2.109876	203.030832	4.286605
2.115139	212.527659	4.291610
2.088452	204.736161	4.296614
2.016712	203.719091	4.301619
1.887461	210.402228	4.306624
2.036280	207.841467	4.311629
2.193886	206.984618	4.316634
2.410892	199.151776	4.321638
1.939326	185.475723	4.326643
1.852854	189.073777	4.331648
2.044929	179.046011	4.336653
1.758887	188.053786	4.341658
2.017029	191.132767	4.346662
2.108684	182.936753	4.351667
1.720628	186.683301	4.356672
1.637587	197.342413	4.361677
1.753961	206.116300	4.366682
1.855046	201.342032	4.371686
1.779951	202.536983	4.376691
1.660850	209.911402	4.381696
2.272739	199.773555	4.386701
1.889528	208.394762	4.391706
1.785585	202.807883	4.396710
1.995127	202.189672	4.401715
1.841489	203.877827	4.406720
2.553239	209.521184	4.411725
1.951674	225.772898	4.416730
2.362935	220.589352	4.421734
2.074870	213.506365	4.426739
2.096708	225.626557	4.431744
2.360206	220.564241	4.436749
2.227451	234.467734	4.441754
2.489156	236.204712	4.446758
2.482864	221.683763	4.451763
2.025852	218.528214	4.456768
1.711854	211.898551	4.461773
2.230561	219.536879	4.466778
2.508010	226.630870	4.471782
2.641121	229.352956	4.476787
2.404948	231.591891	4.481792
2.320989	225.663347	4.486797
2.295473	231.381098	4.491802
2.661586	228.238950	4.496806
2.285155	223.083906	4.501811
2.112279	225.116767	4.506816
2.215804	221.031821	4.511821
2.385041	238.472589	4.516826
2.569429	227.968266	4.521830
2.775850	228.239573	4.526835
2.648835	233.448037	4.531840
2.797147	224.831832	4.536845
2.308971	215.024526	4.541850
2.068924	216.229504	4.546854
2.430610	227.508662	4.551859
2.325485	235.209938	4.556864
2.465144	229.546916	4.561869
2.150313	236.578685	4.566874
2.425341	229.878872	4.571878
2.492811	231.709559	4.576883
2.612534	229.716511	4.581888
2.592824	234.961947	4.586893
2.398480	231.088186	4.591898
2.769166	234.010334	4.596902
2.468202	236.870036	4.601907
2.474545	231.566429	4.606912
2.870124	235.471784	4.611917
2.672086	241.985374	4.616922
2.622847	228.954973	4.621926
2.999866	233.350462	4.626931
2.741984	238.089041	4.631936
2.497634	230.546774	4.636941
2.673684	238.646929	4.641946
2.501380	239.107291	4.646950
2.559609	230.071757	4.651955
2.727716	231.994245	4.656960
2.857255	236.289302	4.661965
2.771551	246.705248	4.666970
2.854883	227.095506	4.671974
2.612516	231.009064	4.676979
2.639327	238.110692	4.681984
3.384763	239.370076	4.686989
2.664131	242.257567	4.691994
3.028266	234.718038	4.696998
3.217032	230.240077	4.702003
2.879481	234.295101	4.707008
3.305880	226.261758	4.712013
2.694107	227.790738	4.717018
2.823151	226.650457	4.722022
2.879243	224.031455	4.727027
2.591952	238.104699	4.732032
2.921910	234.439860	4.737037
2.895180	245.583731	4.742042
3.027931	256.095171	4.747046
3.411788	250.672297	4.752051
2.660720	242.453268	4.757056
2.967143	247.084451	4.762061
3.110642	256.879187	4.767066
3.241544	258.019719	4.772070
3.151099	248.570864	4.777075
2.627896	248.190848	4.782080
2.989151	241.056735	4.787085
3.014480	262.474833	4.792090
3.245393	255.535146	4.797094
3.444818	253.947230	4.802099
3.142526	261.603477	4.807104
3.375592	261.497280	4.812109
3.188200	256.572040	4.817114
3.291309	250.962196	4.822118
3.100069	242.165063	4.827123
2.976663	248.508772	4.832128
2.938631	261.049663	4.837133
3.122326	256.645257	4.842138
3.322195	250.099585	4.847142
3.634538	250.604237	4.852147
2.843596	254.224094	4.857152
3.303788	245.011675	4.862157
3.200907	262.362223	4.867162
3.259426	261.530388	4.872166
3.444941	260.555266	4.877171
2.973615	259.031314	4.882176
3.218557	254.025681	4.887181
3.501966	251.988001	4.892186
3.155508	254.576418	4.897190
3.444453	253.249728	4.902195
3.063049	256.751634	4.907200
3.311131	251.033652	4.912205
2.785618	262.986525	4.917210
3.016330	250.877206	4.922214
3.662829	265.357831	4.927219
3.570304	278.489414	4.932224
3.737782	280.813810	4.937229
3.267362	275.119810	4.942234
2.925558	269.260125	4.947238
3.153274	281.351261	4.952243
3.580814	276.177803	4.957248
3.787470	279.407239	4.962253
3.557439	283.711188	4.967258
3.420843	285.374533	4.972262
3.772045	283.566678	4.977267
3.692926	288.524039	4.982272
3.958085	281.642252	4.987277
3.999025	281.265596	4.992282
3.796195	273.153646	4.997286
3.896345	266.822912	5.002291
3.496404	263.269264	5.007296
3.382126	252.856016	5.012301
3.452151	269.072146	5.017306
3.616967	275.006867	5.022310
3.495954	281.277445	5.027315
3.474982	280.907325	5.032320
3.805722	287.676610	5.037325
3.616312	282.501737	5.042330
3.526278	279.725285	5.047334
3.874066	274.035967	5.052339
3.477008	285.709296	5.057344
4.098233	279.189344	5.062349
3.512663	279.293672	5.067354
3.507612	290.136776	5.072358
3.616458	276.268471	5.077363
3.455237	283.908953	5.082368
3.492177	280.391256	5.087373
3.358271	301.524296	5.092378
3.789875	306.003000	5.097382
4.114507	306.565841	5.102387
3.969942	309.170091	5.107392
4.072068	308.312438	5.112397
4.254420	314.522840	5.117402
4.038130	306.340217	5.122406
4.234971	291.711452	5.127411
3.659235	287.141285	5.132416
3.861800	289.127984	5.137421
4.040693	302.470163	5.142426
4.168183	306.366917	5.147430
4.122001	299.647803	5.152435
3.898521	301.774024	5.157440
4.065820	289.462640	5.162445
3.740344	290.143159	5.167450
3.666395	300.826219	5.172454
4.161338	301.163054	5.177459
4.045624	313.972423	5.182464
4.338124	311.107556	5.187469
4.259301	309.689784	5.192474
4.394132	306.830638	5.197478
4.445927	307.879161	5.202483
4.009120	288.939318	5.207488
4.133085	293.890172	5.212493
4.199921	305.130155	5.217498
4.225121	303.028519	5.222502
4.569740	309.678577	5.227507
3.954501	300.565026	5.232512
4.044963	285.332826	5.237517
4.071531	299.347451	5.242522
4.453409	305.384216	5.247526
4.502986	308.941995	5.252531
4.351548	307.510290	5.257536
4.257431	295.119636	5.262541
4.258614	292.211828	5.267546
4.250470	289.533277	5.272550
4.543499	289.468306	5.277555
4.205122	300.097882	5.282560
4.312927	304.377378	5.287565
4.451452	315.125234	5.292570
4.302247	307.514242	5.297574
4.708944	302.258620	5.302579
4.415781	294.224091	5.307584
4.163037	285.256236	5.312589
4.364693	295.487979	5.317594
4.326802	306.247651	5.322598
4.465677	306.440956	5.327603
4.457996	312.690624	5.332608
4.822178	301.636057	5.337613
4.391216	300.352555	5.342618
4.517222	301.433744	5.347622
4.724514	299.967981	5.352627
4.203353	301.707401	5.357632
4.052180	302.746596	5.362637
4.395381	312.658772	5.367642
4.294931	310.149708	5.372646
4.324168	308.117043	5.377651
4.221535	315.757850	5.382656
4.148877	319.787209	5.387661
4.114860	314.230468	5.392666
4.492066	328.968478	5.397670
4.696627	328.892057	5.402675
4.494819	339.728054	5.407680
4.399112	335.016222	5.412685
4.773245	340.478398	5.417690
4.775558	337.665320	5.422694
4.776951	338.835641	5.427699
4.681410	342.789494	5.432704
4.510231	333.068500	5.437709
4.415442	341.730004	5.442714
4.599911	344.137169	5.447718
4.691940	328.341526	5.452723
4.810629	337.630818	5.457728
4.770872	332.413501	5.462733
4.985810	340.719585	5.467738
4.566257	328.183740	5.472742
4.769675	337.678061	5.477747
4.720995	335.739861	5.482752
4.638785	334.882614	5.487757
4.358697	333.901344	5.492762
4.609786	340.167426	5.497766
4.964305	348.011872	5.502771
4.982608	360.990106	5.507776
4.963962	354.465978	5.512781
4.923164	355.402459	5.517786
5.017475	354.751677	5.522790
4.976079	345.098928	5.527795
5.207579	359.483298	5.532800
5.059223	339.890751	5.537805
4.803052	352.984752	5.542810
4.926883	343.208038	5.547814
5.088013	342.594245	5.552819
4.741792	353.484515	5.557824
5.235314	353.242594	5.562829
5.219580	359.531506	5.567834
5.019118	352.036096	5.572838
5.109468	348.383465	5.577843
5.049480	356.207437	5.582848
5.244935	354.851094	5.587853
4.952985	354.456989	5.592858
5.090269	356.333699	5.597862
4.891448	352.198015	5.602867
4.522329	360.257090	5.607872
4.905536	361.067025	5.612877
5.004034	360.611744	5.617882
4.825029	359.902543	5.622886
5.177466	350.273509	5.627891
5.039617	365.364337	5.632896
4.926241	355.931673	5.637901
4.993956	364.343095	5.642906
4.885895	379.413449	5.647910
5.465691	382.068734	5.652915
5.465394	387.048575	5.657920
5.421445	391.070288	5.662925
5.491777	395.963133	5.667930
5.434721	380.143346	5.672934
5.380694	364.047845	5.677939
5.421733	367.116579	5.682944
5.126948	350.755085	5.687949
5.170016	370.544327	5.692954
5.081008	377.926755	5.697958
5.289375	375.166811	5.702963
5.055455	388.529441	5.707968
5.305985	377.922916	5.712973
5.335801	384.369219	5.717978
5.146486	386.499589	5.722982
5.494728	382.050388	5.727987
5.482460	381.621953	5.732992
5.541097	379.271455	5.737997
5.365521	383.484637	5.743002
5.980645	388.108619	5.748006
5.945919	377.755601	5.753011
5.726065	382.693909	5.758016
5.635322	378.977894	5.763021
5.839669	382.119123	5.768026
5.574725	373.339801	5.773030
5.885707	384.285310	5.778035
5.468061	384.856884	5.783040
5.741926	378.350192	5.788045
5.579479	365.302627	5.793050
5.502757	375.745715	5.798054
5.837677	378.018578	5.803059
5.486044	383.879226	5.808064
5.603893	372.572139	5.813069
5.654147	383.131382	5.818074
5.852162	383.938696	5.823078
5.905176	385.550195	5.828083
5.541285	380.794947	5.833088
5.694692	382.131282	5.838093
5.470173	383.545814	5.843098
5.564247	380.585472	5.848102
6.082350	384.740588	5.853107
5.248248	386.829612	5.858112
6.128459	377.981597	5.863117
6.239556	383.820365	5.868122
5.663874	381.698969	5.873126
5.491730	377.549609	5.878131
5.395122	379.137093	5.883136
5.545648	391.591583	5.888141
5.836659	383.997008	5.893146
5.556900	387.710810	5.898150
5.855194	376.903808	5.903155
5.580578	392.610888	5.908160
5.744635	388.712576	5.913165
6.264562	390.934307	5.918170
6.013145	382.092748	5.923174
5.930985	380.276851	5.928179
5.687007	389.974179	5.933184
6.095200	381.304525	5.938189
6.283685	392.819739	5.943194
5.895384	388.039839	5.948198
5.766743	390.068952	5.953203
5.561257	399.048391	5.958208
5.733930	405.339438	5.963213
6.137474	410.252847	5.968218
5.990355	406.820913	5.973222
6.377265	409.228007	5.978227
6.261668	421.373029	5.983232
6.188168	409.735222	5.988237
6.036645	412.112781	5.993242
6.055399	399.767646	5.998246
6.068764	379.994688	6.003251
5.852202	397.413800	6.008256
6.380706	396.619055	6.013261
6.113745	390.801388	6.018266
5.604179	392.266910	6.023270
5.946842	397.904881	6.028275
6.226424	406.957024	6.033280
5.938197	410.039389	6.038285
6.045480	407.225674	6.043290
5.865373	413.644765	6.048294
6.174408	408.777747	6.053299
6.267120	416.682227	6.058304
6.478358	398.972705	6.063309
6.057922	389.695705	6.068314
5.539680	389.017508	6.073318
5.943987	392.832943	6.078323
5.950231	408.508687	6.083328
6.145279	401.970042	6.088333
6.355509	413.908980	6.093338
6.035459	402.660993	6.098342
6.333076	395.138147	6.103347
6.012869	390.414017	6.108352
5.869901	386.608105	6.113357
5.847410	380.919821	6.118362
5.713943	391.530001	6.123366
5.932347	404.473750	6.128371
6.418240	405.998444	6.133376
6.494071	403.749656	6.138381
6.162984	398.935478	6.143386
5.698094	388.380927	6.148390
6.103809	379.313019	6.153395
5.886903	388.635936	6.158400
5.749014	387.739954	6.163405
6.059637	388.051886	6.168410
6.093675	402.122370	6.173414
6.386379	398.428532	6.178419
6.114141	402.093701	6.183424
5.742138	395.137691	6.188429
5.882360	391.353848	6.193434
5.701128	403.021911	6.198438
6.119774	407.078717	6.203443
6.116517	409.622875	6.208448
5.957122	409.321898	6.213453
6.317474	410.432817	6.218458
5.885004	412.158351	6.223462
6.089795	405.412529	6.228467
6.148644	415.062423	6.233472
6.168988	413.249445	6.238477
5.923239	411.278838	6.243482
6.035588	410.542968	6.248486
6.307096	410.465549	6.253491
5.861823	402.878758	6.258496
5.832932	402.921175	6.263501
6.349963	405.579970	6.268506
5.710999	412.627791	6.273510
5.805441	402.719604	6.278515
6.121327	409.643128	6.283520
6.217462	406.631837	6.288525
6.386321	410.484166	6.293530
6.042966	411.354157	6.298534
5.873202	394.302301	6.303539
5.725386	408.119702	6.308544
5.612577	413.401924	6.313549
6.391480	412.662860	6.318554
6.149745	421.730251	6.323558
6.676658	406.768094	6.328563
5.848459	403.901629	6.333568
5.869896	394.330761	6.338573
5.951489	403.480363	6.343578
5.785674	411.520262	6.348582
6.116163	403.590455	6.353587
6.140511	413.476714	6.358592
5.927110	408.508049	6.363597
6.096012	411.202408	6.368602
6.142410	409.980149	6.373606
6.044952	412.624491	6.378611
6.197800	416.365432	6.383616
6.584059	405.506664	6.388621
6.279260	390.105345	6.393626
5.785557	389.189179	6.398630
5.929783	378.469592	6.403635
5.763755	385.436975	6.408640
5.636496	385.346104	6.413645
6.237977	394.765430	6.418650
6.019252	409.011568	6.423654
6.269802	405.865349	6.428659
6.113844	404.902592	6.433664
5.717804	404.031237	6.438669
6.204839	406.485920	6.443674
6.135632	412.182100	6.448678
6.261845	410.710048	6.453683
6.063401	403.245938	6.458688
5.791003	392.022130	6.463693
6.093129	393.689514	6.468698
5.930438	397.625427	6.473702
6.102179	398.496971	6.478707
6.165141	404.634360	6.483712
5.995978	381.454075	6.488717
5.929110	386.757566	6.493722
5.584856	404.421323	6.498726
6.322026	405.315010	6.503731
6.222073	406.308220	6.508736
6.148414	408.483748	6.513741
6.409390	394.338409	6.518746
6.207319	390.057689	6.523750
6.345912	388.675450	6.528755
5.836219	386.537388	6.533760
5.995711	383.630072	6.538765
6.217541	385.009472	6.543770
6.196570	384.636185	6.548774
5.946507	385.510541	6.553779
5.944633	383.574494	6.558784
5.888292	386.032051	6.563789
6.148403	386.468959	6.568794
5.907265	389.417390	6.573798
6.364466	384.058916	6.578803
6.226783	395.603089	6.583808
6.455818	384.715183	6.588813
6.136574	382.135983	6.593818
6.131149	392.656497	6.598822
6.227377	383.890185	6.603827
6.100602	383.043083	6.608832
6.110333	376.748623	6.613837
6.111864	388.568380	6.618842
6.180300	400.681389	6.623846
6.139738	387.004091	6.628851
6.016698	385.757760	6.633856
6.120834	386.880347	6.638861
6.168619	394.023045	6.643866
5.596781	390.641841	6.648870
6.230096	385.021650	6.653875
5.779008	392.277313	6.658880
5.653022	395.853125	6.663885
6.256618	381.334567	6.668890
5.685669	385.385064	6.673894
6.088714	382.512356	6.678899
5.499124	384.430189	6.683904
5.842640	386.005663	6.688909
6.123561	374.600257	6.693914
5.658721	385.154783	6.698918
5.687937	379.521674	6.703923
5.786095	389.171723	6.708928
5.841825	409.129870	6.713933
6.175120	403.300410	6.718938
5.971971	406.103683	6.723942
6.270703	405.563243	6.728947
5.849563	416.547549	6.733952
5.895646	412.098227	6.738957
5.836646	414.518238	6.743962
5.544003	417.863895	6.748966
5.868177	418.493252	6.753971
6.155936	418.261423	6.758976
5.877871	410.230804	6.763981
6.048744	410.697514	6.768986
6.058371	417.463376	6.773990
6.184297	417.209445	6.778995
6.332829	416.515364	6.784000
6.405484	412.691481	6.789005
6.371144	416.562994	6.794010
5.618870	414.801466	6.799014
6.187907	414.345227	6.804019
6.263713	406.148430	6.809024
6.050773	407.754144	6.814029
6.185993	408.833896	6.819034
6.134644	408.161641	6.824038
6.284935	407.163556	6.829043
5.903824	396.785703	6.834048
6.040054	396.916147	6.839053
5.935191	395.518267	6.844058
5.624529	409.838923	6.849062
6.169532	412.891981	6.854067
5.922272	417.372672	6.859072
5.987714	409.765971	6.864077
6.425710	416.040761	6.869082
6.337750	415.326784	6.874086
5.955237	391.259238	6.879091
5.557408	402.322143	6.884096
5.985513	413.382200	6.889101
6.462175	413.019531	6.894106
6.254284	410.739264	6.899110
5.891827	404.398703	6.904115
5.666703	398.239112	6.909120
5.859297	406.463304	6.914125
6.218057	412.256949	6.919130
6.173356	419.926690	6.924134
6.331036	406.933343	6.929139
6.087151	402.950245	6.934144
5.655162	400.499441	6.939149
6.288080	409.170349	6.944154
5.773709	419.814915	6.949158
6.328989	412.384572	6.954163
6.399544	408.905877	6.959168
6.164739	399.400465	6.964173
5.911684	396.617898	6.969178
5.588434	392.840231	6.974182
6.058653	404.077186	6.979187
6.362516	408.484181	6.984192
5.879606	392.623535	6.989197
6.028867	391.113071	6.994202
5.980430	403.041909	6.999206
5.959813	401.744727	7.004211
6.088772	414.060240	7.009216
6.137454	417.482135	7.014221
6.235448	408.395987	7.019226
6.171609	397.142662	7.024230
5.881493	393.505340	7.029235
5.768301	396.341974	7.034240
6.166208	408.887434	7.039245
5.961601	417.177029	7.044250
5.921007	413.848629	7.049254
5.857880	415.095504	7.054259
6.416568	411.562474	7.059264
6.122986	411.212917	7.064269
6.227912	401.758681	7.069274
5.739603	401.196019	7.074278
5.950132	401.827363	7.079283
6.025721	411.844801	7.084288
5.974348	420.433099	7.089293
6.342068	414.734287	7.094298
6.154874	417.117435	7.099302
6.159018	408.286443	7.104307
6.188392	395.911172	7.109312
6.024944	385.078433	7.114317
6.052463	388.408723	7.119322
5.739494	392.130893	7.124326
5.720001	391.801669	7.129331
6.061239	393.864731	7.134336
6.176739	416.604023	7.139341
6.230698	405.613818	7.144346
5.973855	409.121548	7.149350
5.968444	395.837379	7.154355
5.891622	398.554417	7.159360
6.118197	405.226170	7.164365
6.089263	408.353332	7.169370
6.234313	415.050517	7.174374
5.898715	404.690840	7.179379
5.932833	406.821007	7.184384
6.080337	408.610697	7.189389
5.943180	409.033918	7.194394
6.112906	408.153014	7.199398
6.093915	411.316585	7.204403
5.995595	411.186377	7.209408
6.120327	403.035701	7.214413
6.091367	395.076793	7.219418
5.697805	402.317119	7.224422
6.278827	407.240686	7.229427
6.101732	417.490713	7.234432
6.037142	411.166756	7.239437
6.220264	401.703431	7.244442
5.917050	394.913819	7.249446
6.103697	399.392961	7.254451
5.721613	404.457936	7.259456
5.853808	410.945157	7.264461
6.151739	406.007111	7.269466
5.827243	423.357736	7.274470
6.196133	417.032300	7.279475
6.016990	414.883572	7.284480
5.906364	423.512795	7.289485
6.102722	415.638800	7.294490
6.416713	419.927148	7.299494
6.124674	409.424598	7.304499
6.372263	404.057831	7.309504
5.827380	401.390591	7.314509
5.703868	393.161753	7.319514
5.857449	417.929425	7.324518
6.313086	420.414340	7.329523
6.296630	422.577743	7.334528
5.992471	421.318658	7.339533
6.349260	390.782293	7.344538
5.998156	389.369210	7.349542
5.792921	392.704331	7.354547
6.040821	395.712185	7.359552
6.134223	400.095204	7.364557
6.005571	388.222437	7.369562
5.698031	400.796161	7.374566
6.209782	405.445836	7.379571
6.348117	418.076266	7.384576
5.975513	411.462039	7.389581
5.919322	399.052714	7.394586
6.122868	410.651004	7.399590
6.263146	400.972924	7.404595
6.277307	387.318690	7.409600
5.933126	390.697728	7.414605
6.051012	379.529840	7.419610
5.877427	394.540868	7.424614
5.836474	390.431062	7.429619
6.127910	392.913226	7.434624
5.754198	384.018059	7.439629
6.352728	395.057730	7.444634
5.740097	401.709105	7.449638
6.135017	409.303633	7.454643
6.037498	420.639044	7.459648
5.788018	419.491618	7.464653
6.128418	412.734037	7.469658
5.975339	414.795456	7.474662
6.250053	414.733354	7.479667
6.338109	420.167609	7.484672
6.268715	413.170507	7.489677
6.064139	402.546686	7.494682
5.802541	400.141954	7.499686
5.750636	394.799968	7.504691
5.828076	408.825691	7.509696
6.020982	415.569164	7.514701
6.281678	413.765984	7.519706
6.279303	415.617125	7.524710
6.258355	403.629394	7.529715
6.040361	393.276607	7.534720
6.115043	399.538711	7.539725
6.372100	387.020203	7.544730
5.812192	397.263756	7.549734
5.816765	399.357421	7.554739
5.727774	393.208141	7.559744
5.736978	406.820601	7.564749
6.547861	409.816180	7.569754
5.913481	404.052913	7.574758
6.086359	399.438190	7.579763
5.845295	395.381884	7.584768
5.821056	401.757567	7.589773
6.438268	412.708898	7.594778
5.736551	410.088377	7.599782
6.080858	412.869152	7.604787
5.929557	415.445998	7.609792
5.957046	419.905789	7.614797
6.483695	410.828409	7.619802
6.076417	404.156340	7.624806
5.802752	395.036679	7.629811
6.036536	405.712716	7.634816
6.164610	410.371886	7.639821
6.322876	401.349065	7.644826
5.933240	396.667451	7.649830
6.136371	393.886177	7.654835
6.034523	387.102983	7.659840
5.774187	394.597686	7.664845
5.872734	394.259458	7.669850
6.141856	403.025329	7.674854
6.050701	413.844034	7.679859
6.298801	417.952875	7.684864
6.465415	409.371680	7.689869
6.184858	397.753667	7.694874
5.864781	397.484194	7.699878
6.089394	392.440577	7.704883
5.867324	391.956427	7.709888
5.674957	394.188519	7.714893
5.712654	388.088995	7.719898
5.774831	400.721854	7.724902
6.003616	402.115984	7.729907
6.183960	406.991596	7.734912
5.774521	409.998038	7.739917
6.337665	411.260686	7.744922
6.218010	416.740139	7.749926
6.272602	404.484301	7.754931
5.813530	398.573342	7.759936
5.811673	413.098724	7.764941
6.010156	412.115234	7.769946
6.168669	416.522857	7.774950
6.121335	418.317765	7.779955
5.982124	415.779957	7.784960
6.083896	413.062019	7.789965
6.322866	414.865853	7.794970
6.057724	418.691269	7.799974
6.257218	405.618603	7.804979
6.163096	396.663805	7.809984
5.832036	393.510636	7.814989
6.047600	393.068651	7.819994
5.885436	404.303446	7.824998
6.030711	406.267497	7.830003
6.353118	396.079981	7.835008
5.815185	395.578879	7.840013
5.982191	390.496832	7.845018
6.060723	401.054818	7.850022
5.962034	410.659789	7.855027
6.509607	414.361030	7.860032
6.120210	410.486153	7.865037
6.274266	395.743781	7.870042
5.914795	400.783065	7.875046
5.760313	394.726305	7.880051
6.088334	386.379266	7.885056
5.961632	390.312702	7.890061
6.001276	391.458049	7.895066
5.725649	393.975276	7.900070
5.912202	403.785494	7.905075
6.092162	407.927156	7.910080
6.032987	411.340639	7.915085
5.806260	413.315518	7.920090
6.068042	413.837589	7.925094
6.232600	411.296480	7.930099
6.427848	408.000733	7.935104
6.187897	409.430341	7.940109
6.011976	395.264867	7.945114
5.849282	390.209167	7.950118
5.855543	396.209900	7.955123
6.176478	403.534437	7.960128
5.893389	412.544944	7.965146
6.177510	410.423858	7.970163
6.143369	418.116576	7.975181
6.134221	406.378486	7.980198
5.895700	400.394585	7.985216
5.889505	405.829704	7.990234
6.447907	406.644685	7.995251
6.042847	410.873684	8.000269
5.984951	400.478125	8.005286
5.983935	399.613529	8.010304
5.887977	414.059797	8.015322
6.522246	414.209648	8.020339
5.808939	405.444167	8.025357
6.238526	407.693114	8.030374
6.017934	406.234924	8.035392
5.976304	408.819629	8.040410
6.419878	410.018671	8.045427
6.064106	410.970575	8.050445
6.186606	417.348042	8.055462
6.321448	415.067310	8.060480
6.114262	408.377916	8.065498
5.954751	387.751521	8.070515
5.899934	409.017251	8.075533
6.305744	414.589789	8.080550
6.409655	405.794094	8.085568
6.315677	400.254598	8.090586
6.104459	392.442391	8.095603
5.836338	395.659020	8.100621
6.093152	405.843379	8.105638
6.099805	402.247845	8.110656
6.027501	416.182331	8.115674
6.292202	405.679421	8.120691
6.487529	420.035874	8.125709
6.263406	416.665842	8.130726
6.217683	410.557056	8.135744
5.841769	405.853830	8.140762
6.084307	410.830262	8.145779
6.134966	416.871851	8.150797
6.245099	415.933035	8.155814
6.208177	412.306458	8.160832
6.249845	415.818532	8.165850
6.305157	414.478056	8.170867
6.236205	416.577900	8.175885
5.755468	421.093309	8.180902
6.217368	412.348817	8.185920
6.163899	414.465170	8.190938
6.261622	410.568191	8.195955
6.412745	418.247660	8.200973
5.984025	419.583375	8.205990
6.237066	409.751311	8.211008
6.269958	419.917114	8.216026
6.241164	417.769316	8.221043
6.234447	427.452186	8.226061
5.885066	423.315991	8.231078
6.350952	418.992102	8.236096
6.195457	429.648169	8.241114
5.887201	430.441152	8.246131
6.162166	438.514632	8.251149
6.240567	447.404700	8.256166
6.670106	438.640020	8.261184
6.519949	447.808893	8.266202
6.480904	443.728211	8.271219
6.483611	440.972723	8.276237
6.749614	439.832761	8.281254
6.832836	426.477055	8.286272
6.405789	429.592361	8.291290
6.557960	415.730404	8.296307
6.348028	415.602276	8.301325
6.110725	423.206908	8.306342
6.052890	411.407017	8.311360
6.251929	424.749892	8.316378
6.258970	424.439448	8.321395
6.467904	438.292017	8.326413
6.441666	437.870023	8.331430
6.571375	429.830815	8.336448
6.093961	433.679839	8.341466
6.513835	435.696784	8.346483
6.681332	434.988818	8.351501
6.546778	430.471829	8.356518
6.291451	415.149483	8.361536
6.485536	434.555369	8.366554
6.137244	435.076917	8.371571
7.141575	436.137608	8.376589
6.684374	420.070569	8.381606
6.828654	413.872053	8.386624
6.062748	418.208083	8.391642
6.571946	408.884988	8.396659
6.076057	406.523202	8.401677
6.102868	424.364780	8.406694
6.449062	434.424699	8.411712
6.263240	437.997667	8.416730
6.438736	443.085597	8.421747
6.585907	439.865666	8.426765
6.340585	439.575827	8.431782
7.221700	439.633355	8.436800
6.724834	442.854275	8.441818
6.492067	430.488495	8.446835
6.546852	432.338583	8.451853
6.623056	449.042681	8.456870
6.695856	428.752222	8.461888
6.494234	419.269097	8.466906
6.325473	434.660896	8.471923
6.630309	435.771225	8.476941
6.614024	443.221317	8.481958
6.355084	441.535606	8.486976
6.772820	440.138343	8.491994
6.964120	440.114605	8.497011
6.892312	430.617447	8.502029
6.549798	422.147308	8.507046
6.565292	410.484249	8.512064
5.936452	420.605412	8.517082
6.193988	432.979775	8.522099
7.092554	429.329696	8.527117
6.895871	437.530722	8.532134
6.970981	435.483406	8.537152
6.695096	431.575533	8.542170
6.286581	427.754712	8.547187
6.657912	428.782040	8.552205
6.439068	441.562404	8.557223
6.756825	434.992721	8.562240
6.709775	438.588127	8.567258
6.701734	437.244952	8.572275
6.408243	438.420626	8.577293
6.663137	438.771928	8.582311
6.862438	435.780513	8.587328
6.579432	435.430308	8.592346
6.814476	440.654072	8.597363
7.077608	442.266392	8.602381
6.814622	444.825826	8.607399
6.938713	449.303281	8.612416
7.006106	452.221202	8.617434
6.670209	438.419919	8.622451
6.263465	430.417426	8.627469
6.475861	439.056125	8.632487
6.762641	439.099478	8.637504
6.682935	443.476320	8.642522
6.362856	452.315218	8.647539
6.693071	443.266299	8.652557
6.559072	442.766515	8.657575
6.530575	443.446239	8.662592
6.156865	448.222594	8.667610
6.336813	454.234471	8.672627
6.976827	454.222478	8.677645
6.961916	465.550809	8.682663
7.068178	455.899507	8.687680
6.873413	453.001389	8.692698
6.501997	459.383676	8.697715
6.779054	457.077501	8.702733
6.771999	467.864965	8.707751
7.089912	465.044308	8.712768
7.460775	456.752711	8.717786
7.019915	453.943644	8.722803
7.172628	446.692923	8.727821
6.993617	441.772646	8.732839
6.610505	448.469182	8.737856
6.683897	449.218148	8.742874
6.992238	448.873118	8.747891
6.978994	436.567611	8.752909
6.912723	448.049144	8.757927
6.565527	445.736638	8.762944
6.873222	444.334526	8.767962
6.846015	442.432627	8.772979
7.167400	445.061446	8.777997
6.853954	449.607455	8.783015
6.795796	448.496192	8.788032
6.883971	436.345207	8.793050
6.882599	437.901140	8.798067
6.943052	435.893989	8.803085
6.553219	444.923691	8.808103
6.899655	461.124719	8.813120
7.038790	463.081513	8.818138
6.775655	471.706373	8.823155
7.428383	467.211187	8.828173
7.101262	468.123891	8.833191
6.875395	453.708916	8.838208
6.967450	456.446250	8.843226
7.281482	459.893568	8.848243
6.976858	446.368243	8.853261
6.806070	446.369680	8.858279
7.053436	460.497109	8.863296
7.323090	461.672911	8.868314
7.078156	454.623345	8.873331
7.066117	446.956629	8.878349
7.185988	437.653494	8.883367
7.046318	437.599563	8.888384
7.004935	437.766915	8.893402
6.754482	440.901890	8.898419
6.975406	441.031300	8.903437
6.830026	454.106272	8.908455
6.985255	458.701926	8.913472
7.093571	461.824873	8.918490
7.039539	458.443962	8.923507
7.277368	462.373430	8.928525
7.085190	471.179674	8.933543
6.865749	468.058205	8.938560
7.162274	465.278768	8.943578
7.277166	459.738086	8.948595
7.142873	453.201354	8.953613
6.832020	463.673502	8.958631
7.048486	456.053030	8.963648
7.261475	461.157181	8.968666
6.604364	465.633965	8.973683
7.255662	460.151248	8.978701
7.030649	469.028907	8.983719
7.071405	469.022445	8.988736
7.273841	460.829818	8.993754
7.146236	471.475228	8.998771
7.225877	468.912807	9.003789
7.272368	472.181142	9.008807
7.450945	476.022067	9.013824
7.205142	467.931225	9.018842
7.115334	472.000392	9.023859
6.924762	462.423996	9.028877
7.145004	470.114748	9.033895
7.317668	470.826070	9.038912
7.159736	471.182095	9.043930
7.231808	473.928875	9.048947
7.293865	475.979797	9.053965
7.176193	471.460152	9.058983
6.968232	477.002644	9.064000
7.629862	472.654384	9.069018
6.913201	471.226576	9.074035
7.464527	468.893206	9.079053
7.423901	470.111313	9.084071
7.069088	465.508905	9.089088
7.412852	458.638496	9.094106
7.200397	467.400578	9.099123
7.396244	456.573914	9.104141
7.508074	457.155913	9.109159
7.520370	466.633855	9.114176
7.271240	468.187584	9.119194
7.016792	476.747970	9.124211
7.377373	462.095937	9.129229
7.307919	471.397344	9.134247
7.406669	469.292672	9.139264
7.271730	467.041580	9.144282
7.256590	475.621274	9.149299
7.334425	470.259962	9.154317
7.397085	473.456337	9.159335
7.191650	472.450198	9.164352
7.149730	485.231275	9.169370
7.268399	493.717429	9.174387
7.809570	493.960763	9.179405
7.735370	485.401217	9.184423
7.412986	488.162465	9.189440
7.728772	467.376302	9.194458
7.131641	474.327285	9.199475
7.343041	475.130367	9.204493
7.377335	484.415526	9.209511
7.293949	490.598061	9.214528
7.550923	492.561642	9.219546
7.202462	490.211459	9.224563
7.438619	488.937316	9.229581
7.890781	494.120767	9.234599
7.671798	494.997595	9.239616
7.560794	490.814568	9.244634
7.503741	487.279491	9.249651
7.494945	490.221979	9.254669
7.412617	487.236812	9.259687
7.346067	497.781155	9.264704
7.426633	494.865138	9.269722
7.109206	490.064363	9.274739
7.321175	489.302091	9.279757
7.891704	498.777791	9.284775
7.870844	506.190757	9.289792
7.736650	491.123920	9.294810
7.552288	498.827587	9.299827
7.658434	498.810879	9.304845
7.561996	489.857187	9.309863
7.436501	494.357980	9.314880
7.985260	496.948025	9.319898
7.725816	503.104502	9.324915
7.585143	489.241034	9.329933
7.602643	485.747925	9.334951
7.535741	493.789788	9.339968
8.011521	496.182986	9.344986
7.645098	488.514974	9.350003
7.511066	480.176242	9.355021
7.069545	478.260360	9.360039
7.422483	493.854489	9.365056
7.875455	490.365732	9.370074
7.482544	488.240263	9.375091
7.581796	490.900736	9.380109
7.416789	492.586453	9.385127
7.138474	493.964878	9.390144
7.492799	490.330632	9.395162
7.413546	492.520461	9.400179
7.809140	497.589700	9.405197
7.818029	488.666843	9.410215
7.643922	494.450187	9.415232
7.817821	495.255990	9.420250
7.642484	493.670782	9.425267
7.503144	496.586388	9.430285
7.804416	494.999087	9.435303
7.528886	495.080051	9.440320
7.597952	491.446318	9.445338
7.858662	514.571984	9.450355
7.652108	512.811786	9.455373
7.818917	516.471528	9.460391
7.649953	527.568418	9.465408
8.109607	517.981632	9.470426
7.961878	521.223602	9.475443
7.540670	503.465659	9.480461
7.701007	510.241171	9.485479
7.555689	515.284714	9.490496
8.077955	518.939256	9.495514
8.098204	519.134822	9.500531
7.852452	521.410701	9.505549
8.276178	514.022817	9.510567
7.611576	497.363359	9.515584
7.757320	489.305832	9.520602
7.870241	506.938343	9.525619
8.025622	507.813319	9.530637
8.008425	509.182391	9.535655
7.809764	508.730607	9.540672
7.807819	499.894647	9.545690
7.775817	502.881798	9.550707
7.827386	521.420177	9.555725
7.977788	516.656548	9.560743
8.340632	524.407032	9.565760
8.103021	502.066527	9.570778
7.935882	499.681622	9.575795
7.583941	493.608163	9.580813
7.786403	503.100510	9.585831
7.552309	523.299409	9.590848
8.088602	513.643814	9.595866
8.040944	524.863705	9.600883
7.843607	514.073364	9.605901
7.886251	512.214162	9.610919
7.896204	526.164248	9.615936
8.200820	524.727898	9.620954
8.134741	527.704613	9.625971
8.263826	522.196402	9.630989
8.151424	524.015890	9.636007
7.856418	523.301491	9.641024
7.805224	520.655421	9.646042
8.254605	513.026834	9.651059
7.654810	519.318693	9.656077
8.000567	515.515372	9.661095
7.689054	524.311937	9.666112
7.917225	516.361404	9.671130
7.886431	513.298731	9.676147
8.251648	521.219254	9.681165
8.355373	518.567846	9.686183
7.982140	521.100383	9.691200
8.022804	519.995723	9.696218
8.155228	516.358370	9.701235
7.982137	515.407121	9.706253
8.469274	520.089641	9.711271
8.102424	524.385262	9.716288
8.311012	512.224827	9.721306
8.158161	518.658095	9.726323
8.033855	519.712593	9.731341
8.210698	514.843836	9.736359
8.315711	519.873404	9.741376
8.068249	517.662027	9.746394
8.431883	516.995910	9.751411
8.115009	522.410315	9.756429
8.283804	516.116404	9.761447
7.989006	518.191686	9.766464
8.003473	519.268621	9.771482
7.956671	514.674745	9.776499
7.937481	517.893419	9.781517
8.358254	511.496915	9.786535
7.976911	520.206590	9.791552
8.059112	520.004287	9.796570
8.128609	525.765253	9.801587
8.445898	525.052748	9.806605
8.230778	524.183823	9.811623
8.019755	525.378139	9.816640
8.185561	535.958681	9.821658
8.363984	539.897474	9.826675
8.108364	553.147580	9.831693
8.627536	543.333706	9.836711
8.443668	539.149461	9.841728
8.455441	538.989751	9.846746
8.336337	529.638805	9.851763
8.033571	535.256130	9.856781
8.226093	543.689711	9.861799
8.428305	544.068205	9.866816
8.299703	544.738370	9.871834
8.391722	545.200401	9.876851
8.376118	550.220474	9.881869
8.484920	540.619220	9.886887
8.657948	537.612970	9.891904
8.446599	539.886617	9.896922
8.626154	544.125034	9.901939
8.493842	547.086883	9.906957
8.151496	522.462193	9.911975
8.237497	532.181085	9.916992
8.284036	538.557874	9.922010
8.301689	540.312805	9.927027
8.093291	542.668041	9.932045
8.325258	542.511700	9.937063
8.607678	551.492930	9.942080
8.698089	552.393867	9.947098
8.693511	546.259654	9.952115
8.534051	551.166568	9.957133
8.546270	542.849073	9.962151
8.907594	545.307548	9.967168
8.729677	547.383455	9.972186
8.693673	533.374166	9.977203
8.289887	535.258244	9.982221
8.554072	519.384199	9.987239
8.364875	526.927690	9.992256
8.317783	537.658354	9.997274
8.274672	534.442974	10.002291
7.964610	548.029809	10.007309
8.123029	542.188793	10.012327
8.005744	541.380277	10.017344
8.208600	536.835640	10.022362
8.074677	551.354239	10.027379
8.334894	560.083334	10.032397
8.641410	561.685711	10.037415
8.484721	567.889226	10.042432
8.766399	569.381887	10.047450
8.751553	566.048464	10.052467
8.444794	577.940144	10.057485
8.954844	570.986834	10.062503
8.950473	574.269468	10.067520
8.883985	576.567759	10.072538
8.945312	568.113171	10.077555
8.673842	553.872517	10.082573
8.523466	548.303942	10.087591
8.690142	566.335186	10.092608
8.739608	572.200290	10.097626
8.900837	571.638467	10.102643
8.726693	557.193214	10.107661
8.584583	554.750731	10.112679
8.931622	554.371234	10.117696
8.839302	553.205357	10.122714
8.875236	547.244675	10.127731
8.614147	548.140726	10.132749
8.644155	547.836148	10.137767
8.943278	549.695301	10.142784
8.836181	553.723014	10.147802
8.566242	546.891922	10.152819
8.436729	555.581093	10.157837
8.806605	569.784087	10.162855
8.679493	572.388521	10.167872
8.859088	572.915725	10.172890
8.665577	577.973148	10.177907
8.607560	583.631035	10.182925
8.540779	578.822523	10.187943
8.605484	578.143281	10.192960
8.361916	583.741877	10.197978
8.673124	586.643710	10.202995
8.536380	585.648892	10.208013
8.229501	586.031412	10.213031
8.603113	598.744309	10.218048
8.891479	606.304526	10.223066
9.140612	607.502489	10.228083
8.689267	612.193221	10.233101
8.794593	606.126973	10.238119
8.927875	606.970704	10.243136
8.709451	609.289649	10.248154
8.985554	603.556406	10.253171
8.951551	609.904815	10.258189
8.916077	612.996669	10.263207
9.065901	606.825620	10.268224
9.066592	607.248313	10.273242
9.182752	601.095163	10.278259
8.874706	600.603710	10.283277
8.985266	613.556647	10.288295
8.959851	601.660033	10.293312
8.891980	615.912715	10.298330
8.962653	609.706729	10.303347
8.705388	616.844357	10.308365
9.254786	612.822917	10.313383
8.928804	606.533914	10.318400
8.726592	613.823860	10.323418
8.910310	602.471989	10.328435
8.832507	618.853239	10.333453
8.774138	612.822105	10.338471
9.322443	611.199245	10.343488
9.095463	620.373932	10.348506
9.225930	606.975975	10.353523
8.844750	614.713684	10.358541
8.811380	623.854882	10.363559
9.423937	623.433782	10.368576
9.207606	629.258499	10.373594
9.246106	625.645308	10.378611
8.883644	630.991149	10.383629
9.424080	632.714672	10.388647
9.218331	613.316558	10.393664
9.220683	619.817063	10.398682
9.023940	618.304626	10.403699
9.263790	622.685092	10.408717
9.000693	624.389346	10.413735
9.366363	626.493701	10.418752
9.113402	627.798736	10.423770
9.358922	627.248952	10.428787
8.711526	622.963744	10.433805
9.178726	629.274656	10.438823
9.278342	633.134299	10.443840
8.920678	638.498325	10.448858
8.997837	643.895210	10.453875
9.372948	643.997307	10.458893
9.301082	644.443992	10.463911
9.695305	633.889096	10.468928
9.097626	638.075744	10.473946
9.201940	643.222221	10.478963
9.410256	642.719291	10.483981
8.993061	644.280433	10.488999
9.139994	639.403706	10.494016
8.890182	644.668784	10.499034
8.952154	644.753673	10.504051
9.250636	641.273313	10.509069
9.120529	648.372095	10.514087
9.329229	653.937722	10.519104
9.348497	671.480927	10.524122
9.677850	660.961426	10.529139
9.573566	662.353621	10.534157
9.392826	657.253674	10.539175
9.268171	645.328398	10.544192
9.544708	653.685752	10.549210
9.430722	647.559179	10.554227
9.041499	654.502902	10.559245
9.367912	665.888334	10.564263
9.775106	663.580678	10.569280
9.043048	673.484625	10.574298
9.532389	668.636292	10.579315
9.351040	678.857901	10.584333
9.438252	678.891497	10.589351
9.685251	673.247999	10.594368
9.528073	673.373536	10.599386
9.798852	670.812696	10.604403
9.696248	673.119815	10.609421
9.483070	671.354327	10.614439
9.516520	662.885127	10.619456
9.405486	675.427860	10.624474
9.536058	670.367495	10.629491
9.662629	670.530624	10.634509
9.393131	666.659568	10.639527
9.606110	656.619052	10.644544
9.179805	664.433280	10.649562
9.222258	665.521618	10.654579
9.187434	669.023636	10.659597
9.451990	659.675626	10.664615
9.396372	659.251918	10.669632
9.697848	667.090974	10.674650
9.711877	669.256742	10.679667
9.803886	674.013835	10.684685
9.464001	680.785736	10.689703
9.318919	671.037999	10.694720
9.621316	674.685997	10.699738
9.909656	686.790622	10.704755
9.971335	676.991551	10.709773
9.407939	670.304221	10.714791
9.946789	657.681686	10.719808
9.929229	670.673673	10.724826
10.041989	661.280018	10.729843
9.867003	655.996133	10.734861
9.376284	665.925379	10.739879
9.411526	665.623135	10.744896
9.151095	671.183375	10.749914
9.580839	687.665046	10.754931
9.763337	689.223750	10.759949
9.819384	694.535596	10.764967
10.126205	692.543465	10.769984
9.858577	694.119046	10.775002
10.087717	694.493324	10.780019
10.196649	686.558243	10.785037
9.847063	686.448837	10.790055
9.860727	676.736184	10.795072
9.829583	672.023050	10.800090
9.656345	672.005935	10.805107
9.677842	672.696769	10.810125
9.829210	687.798786	10.815143
10.048265	682.058677	10.820160
9.903790	687.335666	10.825178
9.944611	680.790349	10.830195
10.492031	677.526600	10.835213
9.967363	676.930230	10.840231
9.787780	666.310584	10.845248
9.633675	671.402885	10.850266
9.768052	674.117843	10.855283
9.785560	675.948550	10.860301
10.111434	691.619676	10.865319
9.953591	678.118515	10.870336
10.139698	683.359486	10.875354
10.266348	687.426345	10.880371
10.200669	685.328476	10.885389
9.751897	680.166376	10.890407
10.058798	679.294547	10.895424
9.915166	691.220703	10.900442
9.811365	692.287776	10.905459
10.287431	691.771296	10.910477
10.044086	694.996720	10.915495
10.129219	683.802256	10.920512
10.113805	691.435352	10.925530
9.703698	696.551991	10.930547
9.905884	690.574681	10.935565
9.651290	696.212910	10.940583
9.923684	689.994226	10.945600
10.047455	692.767653	10.950618
9.917014	702.883468	10.955635
9.955057	699.115698	10.960653
9.874390	691.951937	10.965671
9.944871	689.763306	10.970688
9.727579	698.362157	10.975706
9.956619	708.551040	10.980723
9.896253	714.632216	10.985741
10.145329	718.083450	10.990759
10.373553	720.288247	10.995776
10.305238	715.984870	11.000794
10.499682	723.143284	11.005811
10.632162	721.531918	11.010829
10.546441	723.192610	11.015847
10.165628	704.976855	11.020864
10.277999	698.499217	11.025882
10.387523	700.918270	11.030899
10.528635	693.369465	11.035917
9.940353	690.936909	11.040935
10.041446	683.937178	11.045952
9.904009	697.787414	11.050970
10.352118	713.227968	11.055987
10.754070	714.354657	11.061005
10.372983	718.056104	11.066023
10.286412	706.244742	11.071040
10.750371	712.209051	11.076058
10.024716	710.154624	11.081075
10.407516	703.429484	11.086093
10.323333	715.475731	11.091111
10.430059	712.808045	11.096128
10.218330	718.187099	11.101146
10.567924	720.609567	11.106163
10.567092	717.453801	11.111181
10.417155	725.319429	11.116199
10.610465	713.379003	11.121216
10.790910	698.319498	11.126234
10.353581	701.038828	11.131251
10.382224	693.848472	11.136269
10.379638	699.330452	11.141287
10.513474	697.144517	11.146304
10.575388	703.329607	11.151322
10.388034	702.481568	11.156339
10.586576	697.382144	11.161357
10.451453	707.031634	11.166375
10.365801	719.024464	11.171392
10.766530	717.257459	11.176410
10.404660	719.062405	11.181427
10.426465	718.711772	11.186445
10.588864	717.307158	11.191463
10.944790	720.315616	11.196480
10.894562	713.598359	11.201498
10.666192	706.744914	11.206515
10.400643	699.032603	11.211533
10.473246	707.131599	11.216551
10.795422	718.233706	11.221568
10.779714	713.420311	11.226586
10.344684	709.404767	11.231603
10.759533	715.935352	11.236621
10.697231	723.537939	11.241639
10.729323	723.766365	11.246656
10.205838	712.468425	11.251674
10.414127	728.688185	11.256691
10.830706	719.581414	11.261709
10.609948	729.342164	11.266727
10.189728	721.988594	11.271744
10.754959	720.713369	11.276762
10.477971	727.759456	11.281779
10.707182	716.027999	11.286797
10.804374	717.896718	11.291815
10.681121	734.790126	11.296832
10.551698	728.126298	11.301850
10.621596	733.300285	11.306867
11.119705	714.129453	11.311885
10.846143	721.588413	11.316903
10.459643	723.293076	11.321920
10.659125	725.290937	11.326938
10.354225	732.177297	11.331955
10.552618	737.634111	11.336973
10.973538	742.494324	11.341991
10.926888	745.928782	11.347008
10.866869	747.254088	11.352026
10.864097	741.141616	11.357043
10.919447	745.282775	11.362061
11.073890	748.894010	11.367079
10.956973	744.355242	11.372096
11.037697	743.048630	11.377114
11.198097	749.918898	11.382131
11.346138	740.052612	11.387149
11.055464	724.893330	11.392167
11.029905	725.036114	11.397184
11.289911	715.392142	11.402202
10.965898	727.381298	11.407219
11.113030	716.555798	11.412237
11.223310	719.173552	11.417255
10.722432	722.275228	11.422272
10.783575	715.685689	11.427290
10.666972	715.647077	11.432307
11.105807	728.696987	11.437325
11.225939	732.979473	11.442343
11.204485	731.537392	11.447360
11.281974	727.299530	11.452378
10.839217	725.702552	11.457395
11.042142	717.822158	11.462413
10.819856	728.927526	11.467431
11.103626	743.980443	11.472448
11.197278	737.332153	11.477466
10.976803	745.028959	11.482483
11.033975	740.185204	11.487501
11.176808	746.717394	11.492519
11.232254	741.264835	11.497536
11.386659	741.108022	11.502554
11.076236	745.148699	11.507571
11.180804	741.455705	11.512589
11.139782	745.173304	11.517607
11.250461	749.343666	11.522624
11.233362	737.694968	11.527642
10.884742	741.205140	11.532659
11.169581	738.733607	11.537677
10.777738	744.712093	11.542695
10.865250	747.992986	11.547712
11.196289	745.006126	11.552730
11.160393	748.300042	11.557747
11.076851	739.833357	11.562765
10.881541	750.192894	11.567783
11.394443	763.193354	11.572800
11.455147	770.943947	11.577818
11.564503	768.146453	11.582835
11.536775	772.199649	11.587853
11.371651	768.129179	11.592871
11.637709	754.716178	11.597888
11.463694	752.827781	11.602906
10.950970	743.080801	11.607923
11.139248	748.469775	11.612941
11.577635	764.341089	11.617959
11.761528	769.525628	11.622976
11.628509	760.650115	11.627994
11.306093	747.648061	11.633011
11.573855	752.194601	11.638029
11.445283	747.458841	11.643047
10.931926	749.448472	11.648064
11.455635	765.407405	11.653082
11.506656	772.010794	11.658099
11.494749	773.909237	11.663117
11.614238	763.880152	11.668135
11.642887	771.850364	11.673152
11.611035	774.749174	11.678170
11.721444	768.350713	11.683187
11.509622	768.784615	11.688205
11.961441	769.972923	11.693223
11.551153	772.665936	11.698240
11.598558	749.535690	11.703258
11.784278	757.904167	11.708275
11.623117	761.293452	11.713293
11.892094	744.392814	11.718311
11.682289	745.706874	11.723328
11.487024	730.333822	11.728346
11.616398	742.630650	11.733363
11.324752	736.254169	11.738381
11.457925	741.806411	11.743399
11.616657	763.550347	11.748416
11.879540	752.428976	11.753434
11.899803	766.914124	11.758451
11.837033	766.475755	11.763469
12.085862	763.801577	11.768487
11.459401	753.311857	11.773504
11.668276	745.499947	11.778522
11.743313	761.125228	11.783539
11.722544	764.082260	11.788557
12.445640	755.643818	11.793575
11.706799	753.878632	11.798592
11.525051	739.465981	11.803610
12.084803	745.951783	11.808627
11.502490	750.161294	11.813645
11.724481	754.793902	11.818663
11.906863	761.932131	11.823680
12.167802	761.749159	11.828698
12.104497	759.388975	11.833715
11.950185	760.404006	11.838733
12.080077	744.528712	11.843751
11.871495	737.839413	11.848768
11.797607	729.080885	11.853786
11.688188	741.383568	11.858803
12.010156	756.111772	11.863821
12.426992	748.847949	11.868839
11.924543	750.169991	11.873856
11.790279	727.970803	11.878874
11.753856	743.859687	11.883891
12.112415	748.657089	11.888909
12.387492	747.550401	11.893927
11.775458	747.308545	11.898944
11.939944	736.391951	11.903962
12.280978	746.964098	11.908979
11.825082	753.691086	11.913997
11.854368	752.480896	11.919015
12.037467	756.475810	11.924032
12.077338	761.446224	11.929050
12.298118	759.742124	11.934067
12.195339	776.070626	11.939085
12.377932	769.326337	11.944103
12.019941	769.565389	11.949120
12.072180	764.971710	11.954138
11.901791	766.730880	11.959155
11.822530	768.289578	11.964173
12.011846	763.911109	11.969191
11.761602	769.390888	11.974208
12.316064	773.851488	11.979226
12.394957	769.370397	11.984243
12.358810	770.174409	11.989261
11.923134	775.137285	11.994279
12.046091	774.840231	11.999296
11.961273	765.717320	12.004314
12.156998	772.667270	12.009331
11.924397	767.648001	12.014349
12.209348	765.596172	12.019367
12.267210	776.468326	12.024384
12.276389	768.675071	12.029402
12.782281	770.060035	12.034419
12.124035	772.280654	12.039437
12.444263	766.130189	12.044455
12.095782	772.562641	12.049472
12.405049	772.523576	12.054490
12.545799	767.411096	12.059507
12.159193	771.672001	12.064525
12.468017	773.586464	12.069543
12.271526	783.955672	12.074560
12.517468	778.081931	12.079578
12.354240	777.697172	12.084595
12.346667	785.247028	12.089613
12.882016	788.830149	12.094631
12.471287	784.709794	12.099648
12.295673	779.609009	12.104666
12.526675	777.332100	12.109683
12.432061	792.289707	12.114701
12.734610	791.156621	12.119719
12.510640	787.464599	12.124736
12.302860	784.726258	12.129754
12.571741	788.319571	12.134771
12.892421	787.679110	12.139789
12.923749	776.401499	12.144807
12.386986	774.124963	12.149824
12.388656	758.272902	12.154842
12.719445	769.465210	12.159859
12.510410	779.066360	12.164877
12.850072	771.445386	12.169895
12.673370	771.725462	12.174912
12.371319	771.624387	12.179930
12.894251	762.649255	12.184947
12.433654	767.448775	12.189965
12.959571	775.366323	12.194983
12.635871	782.451309	12.200000
12.277596	779.837535	12.205018
12.553605	777.080200	12.210035
12.207439	787.002643	12.215053
12.707317	783.105690	12.220071
12.519651	791.425387	12.225088
13.000865	790.882850	12.230106
12.717045	786.158782	12.235123
12.627480	777.554165	12.240141
12.406797	782.246671	12.245159
12.672920	779.175301	12.250176
12.874470	791.785906	12.255194
12.887284	782.278458	12.260211
12.845550	782.505828	12.265229
12.226803	787.992857	12.270247
12.861874	808.169506	12.275264
13.159602	806.636384	12.280282
13.263376	801.968348	12.285299
12.998834	792.450702	12.290317
13.368120	781.568264	12.295335
12.864959	786.447042	12.300352
12.531447	784.735111	12.305370
12.698849	797.688743	12.310387
12.604800	806.814295	12.315405
12.992525	811.619768	12.320423
13.210158	803.389890	12.325440
13.391088	799.546062	12.330458
13.615611	807.454042	12.335475
12.692436	790.784329	12.340493
12.963109	786.733937	12.345511
12.991380	789.904198	12.350528
13.010576	796.481025	12.355546
13.168009	794.543847	12.360563
12.819373	807.695105	12.365581
13.274703	801.867446	12.370599
13.295198	800.503994	12.375616
13.095189	811.924663	12.380634
13.505629	797.371843	12.385651
13.363205	787.216522	12.390669
12.819499	788.993160	12.395687
13.075043	792.550693	12.400704
13.095491	800.257113	12.405722
13.724895	796.513434	12.410739
13.396511	800.354965	12.415757
13.023338	789.285892	12.420775
13.252760	789.530739	12.425792
13.239191	789.624307	12.430810
13.160543	791.025120	12.435827
13.059582	801.581344	12.440845
13.387302	807.803719	12.445863
13.300001	795.099311	12.450880
13.187420	786.157467	12.455898
13.514564	804.643496	12.460915
13.253131	805.145133	12.465933
13.302867	800.643356	12.470951
13.058934	807.173050	12.475968
13.341582	814.005254	12.480986
13.413985	811.822619	12.486003
13.156067	815.552125	12.491021
13.470422	816.023509	12.496039
13.665920	821.720646	12.501056
13.428166	805.208617	12.506074
13.886988	802.444726	12.511091
13.338277	805.894741	12.516109
13.787417	803.261756	12.521127
13.600152	806.929698	12.526144
13.358400	798.841226	12.531162
13.535028	795.695513	12.536179
13.327897	808.111382	12.541197
13.419654	812.947448	12.546215
13.695700	806.273711	12.551232
13.616905	811.174369	12.556250
13.866762	803.671596	12.561267
14.037717	805.462495	12.566285
13.531905	783.371945	12.571303
13.218740	789.044627	12.576320
13.388481	800.953315	12.581338
13.571964	803.329236	12.586355
13.581420	806.095345	12.591373
13.759484	809.052789	12.596391
13.850220	817.000671	12.601408
13.656370	817.169823	12.606426
13.433868	806.051886	12.611443
13.287225	806.898458	12.616461
13.197692	809.983038	12.621479
13.709248	813.935969	12.626496
13.570156	814.850787	12.631514
14.110673	814.090674	12.636531
13.692046	808.450437	12.641549
13.309268	809.965175	12.646567
13.842432	811.516285	12.651584
13.380597	811.093103	12.656602
13.701174	820.917411	12.661619
13.756384	830.896912	12.666637
13.633604	830.600489	12.671655
13.652079	836.268562	12.676672
13.689107	833.892648	12.681690
14.064417	832.760783	12.686707
14.060260	836.895508	12.691725
14.150217	842.770136	12.696743
14.096771	830.947189	12.701760
13.965863	831.519895	12.706778
14.060472	829.586245	12.711795
13.937587	827.361621	12.716813
13.999585	821.415700	12.721831
14.131845	824.951530	12.726848
13.970049	825.974049	12.731866
14.339865	824.719968	12.736883
14.181140	827.932157	12.741901
13.903112	819.527464	12.746919
14.039523	823.523396	12.751936
13.800131	835.499366	12.756954
14.161287	825.280902	12.761971
13.945009	830.988910	12.766989
13.892256	822.908686	12.772007
13.951708	826.541131	12.777024
14.081757	826.593263	12.782042
14.404898	823.172122	12.787059
14.017216	831.927123	12.792077
13.938286	833.037646	12.797095
14.143395	832.977031	12.802112
14.092800	826.777346	12.807130
14.276412	822.273524	12.812147
14.179319	822.739944	12.817165
13.882400	826.046370	12.822183
14.430487	828.311519	12.827200
13.987741	836.077904	12.832218
14.161554	823.177928	12.837235
14.166613	828.327387	12.842253
14.219835	837.366764	12.847271
14.592120	823.697224	12.852288
14.106431	830.807610	12.857306
14.466234	833.768142	12.862323
14.526102	821.823304	12.867341
14.228078	820.500289	12.872359
14.477343	829.568906	12.877376
14.184203	833.010442	12.882394
14.364002	824.379379	12.887411
14.350685	834.439047	12.892429
14.278707	847.714248	12.897447
14.424989	848.423407	12.902464
14.663715	845.662436	12.907482
14.379249	844.788580	12.912499
14.840736	854.221595	12.917517
14.527726	850.388874	12.922535
14.843194	844.794556	12.927552
14.498422	836.106820	12.932570
14.098638	830.602481	12.937587
14.424438	843.872160	12.942605
14.634876	854.095599	12.947623
14.920286	841.733553	12.952640
14.586119	858.205683	12.957658
14.572189	851.542648	12.962675
14.746207	852.124384	12.967693
14.360767	858.531100	12.972711
14.567814	843.483084	12.977728
14.734237	846.218294	12.982746
14.823039	848.205108	12.987763
14.480115	856.123121	12.992781
14.536465	853.778892	12.997799
15.073756	849.219648	13.002816
14.588642	854.534278	13.007834
14.671498	848.114860	13.012851
15.041069	850.559462	13.017869
14.814158	858.083754	13.022887
14.899431	841.915560	13.027904
14.806845	846.616414	13.032922
14.914106	843.311146	13.037939
14.942488	844.338583	13.042957
14.484987	861.524324	13.047975
14.936042	837.974109	13.052992
14.690256	838.375464	13.058010
14.787338	839.616201	13.063027
14.882990	840.510020	13.068045
14.842912	848.749814	13.073063
14.945771	833.733910	13.078080
14.886692	844.715948	13.083098
14.701563	844.110554	13.088115
14.905452	844.567687	13.093133
14.605000	847.458099	13.098151
14.972723	834.581383	13.103168
14.638120	844.445240	13.108186
14.874516	851.474056	13.113203
15.174379	859.139878	13.118221
15.094815	866.858841	13.123239
15.418078	857.428946	13.128256
15.034710	852.209210	13.133274
14.901965	842.566744	13.138291
15.098013	855.714748	13.143309
15.316101	872.434883	13.148327
15.860706	856.030603	13.153344
15.290928	846.257792	13.158362
15.659380	835.129297	13.163379
15.485092	824.379338	13.168397
15.725473	839.252939	13.173415
15.600242	834.879555	13.178432
15.126336	830.384075	13.183450
15.380962	837.066042	13.188467
15.250045	823.125046	13.193485
15.201955	835.635938	13.198503
15.202928	820.749618	13.203520
15.118648	830.848806	13.208538
14.898585	830.662301	13.213555
15.193592	829.022304	13.218573
15.067419	837.218777	13.223591
15.321642	830.816696	13.228608
15.310100	834.551786	13.233626
15.288178	840.453410	13.238643
15.388475	825.434758	13.243661
15.479234	833.338462	13.248679
15.252401	830.237021	13.253696
14.798361	833.662741	13.258714
14.946341	843.368935	13.263731
15.054953	854.242653	13.268749
15.126793	848.058493	13.273767
15.450807	861.271659	13.278784
15.468500	860.385175	13.283802
15.322722	856.933355	13.288819
15.920326	857.186789	13.293837
15.763566	862.879170	13.298855
15.858603	861.156891	13.303872
15.876834	859.408777	13.308890
15.771403	857.746310	13.313907
15.721214	857.571059	13.318925
15.411091	866.553769	13.323943
15.646925	856.758871	13.328960
15.774425	861.696649	13.333978
15.775754	859.989052	13.338995
15.807771	849.471846	13.344013
15.640455	857.469644	13.349031
15.839412	854.544487	13.354048
15.833755	856.552413	13.359066
15.537421	853.767975	13.364083
15.692684	860.235143	13.369101
15.590922	851.449363	13.374119
15.844746	853.754309	13.379136
15.741320	853.637892	13.384154
15.715603	865.848650	13.389171
15.724329	855.114180	13.394189
15.946451	853.725445	13.399207
15.863903	861.643691	13.404224
15.611762	868.341954	13.409242
15.649898	854.560641	13.414259
15.912460	866.956609	13.419277
15.526155	865.899890	13.424295
15.744567	877.700017	13.429312
16.335848	880.558016	13.434330
15.983619	883.147273	13.439347
16.157941	883.763677	13.444365
16.198573	888.923359	13.449383
16.407910	878.488807	13.454400
16.014557	862.465014	13.459418
16.020123	858.052196	13.464435
15.796743	856.376651	13.469453
15.650561	859.075634	13.474471
16.486230	871.476487	13.479488
16.041139	879.650362	13.484506
15.903148	879.428906	13.489523
16.467328	877.298601	13.494541
16.438409	888.007693	13.499559
16.682092	876.406409	13.504576
16.404825	860.272909	13.509594
16.200023	858.622856	13.514611
16.086974	848.264081	13.519629
16.279735	857.303695	13.524647
16.365445	856.715826	13.529664
16.355128	858.213237	13.534682
16.145051	860.060686	13.539699
16.332523	849.121486	13.544717
16.192198	853.567887	13.549735
16.371360	852.624545	13.554752
16.455662	842.458917	13.559770
16.176229	860.576134	13.564787
16.129972	858.948578	13.569805
16.320080	869.020575	13.574823
16.215952	875.222272	13.579840
16.211961	878.170382	13.584858
16.306761	885.685306	13.589875
16.516475	877.062154	13.594893
16.321206	884.123901	13.599911
16.655582	883.670643	13.604928
16.860478	873.356712	13.609946
16.790686	878.839810	13.614963
16.648908	873.796812	13.619981
16.476858	873.527043	13.624999
16.337794	870.749520	13.630016
16.527571	876.356051	13.635034
16.676681	885.301532	13.640051
16.590331	881.161889	13.645069
16.713336	881.202501	13.650087
16.564811	879.183863	13.655104
16.933248	873.218314	13.660122
16.287450	873.376226	13.665139
16.476977	875.852197	13.670157
16.545331	872.792863	13.675175
16.773666	878.213471	13.680192
16.455992	881.138145	13.685210
16.291402	877.272697	13.690227
16.637269	878.411340	13.695245
16.775902	881.599040	13.700263
16.698382	879.032782	13.705280
16.660492	874.986535	13.710298
16.577091	876.489085	13.715315
17.041893	888.705057	13.720333
16.669011	887.295934	13.725351
16.976088	895.497136	13.730368
16.968382	896.473425	13.735386
17.221995	897.067939	13.740403
16.824435	880.691333	13.745421
16.920786	876.131740	13.750439
16.767602	887.917511	13.755456
17.086273	887.248959	13.760474
17.122858	895.161177	13.765491
17.029821	879.822472	13.770509
16.693577	883.131914	13.775527
16.873056	893.735773	13.780544
17.137409	893.362913	13.785562
17.162845	897.291042	13.790579
16.858448	900.586029	13.795597
17.210757	902.089744	13.800615
17.138373	899.936095	13.805632
17.364680	901.077693	13.810650
17.277774	899.118826	13.815667
17.109296	892.129691	13.820685
17.208383	885.303767	13.825703
17.047561	896.125050	13.830720
16.989876	894.486658	13.835738
17.227289	897.778806	13.840755
17.396901	885.166626	13.845773
17.498563	893.917571	13.850791
16.903367	895.011155	13.855808
17.158577	892.197100	13.860826
17.153845	904.533987	13.865843
17.032985	899.538199	13.870861
17.354060	893.633713	13.875879
17.467693	889.128215	13.880896
17.299091	899.054457	13.885914
17.192850	893.668210	13.890931
17.199285	893.288424	13.895949
16.961010	892.123302	13.900967
17.389604	898.121618	13.905984
17.577677	893.462442	13.911002
17.379304	899.038276	13.916019
17.302690	896.367730	13.921037
17.061120	902.647777	13.926055
17.229349	908.614306	13.931072
18.129058	921.806747	13.936090
17.708854	921.225558	13.941107
17.912127	920.357331	13.946125
17.850253	905.515502	13.951143
17.445146	906.582459	13.956160
17.494762	896.554780	13.961178
17.390508	907.708039	13.966195
17.838221	909.231521	13.971213
18.100937	920.469304	13.976231
17.836293	914.987947	13.981248
17.653020	907.029121	13.986266
17.733953	908.089354	13.991283
17.486157	893.914148	13.996301
17.782773	904.663764	14.001319
17.877988	907.504816	14.006336
17.893755	898.075740	14.011354
17.721407	911.218389	14.016371
17.591113	913.337370	14.021389
17.864632	917.286594	14.026407
17.833947	920.841662	14.031424
17.883906	914.187529	14.036442
17.953032	922.407090	14.041459
17.947421	925.390177	14.046477
17.915767	923.618313	14.051495
17.755295	926.044986	14.056512
18.304228	913.818329	14.061530
18.283017	919.154970	14.066547
18.019556	918.356716	14.071565
18.528769	905.224246	14.076583
17.972051	910.771022	14.081600
17.741575	894.434497	14.086618
17.683124	905.441721	14.091635
17.806751	913.214076	14.096653
18.542666	910.384662	14.101671
18.091060	919.399034	14.106688
18.215840	918.454742	14.111706
18.132299	923.441382	14.116723
18.517071	919.644487	14.121741
18.438650	909.475913	14.126759
17.926481	899.646708	14.131776
18.094610	906.029824	14.136794
18.584821	911.027553	14.141811
18.607185	902.509483	14.146829
18.434707	893.687424	14.151847
17.830814	893.365393	14.156864
17.879890	888.049489	14.161882
18.443347	901.480793	14.166899
17.844975	907.210822	14.171917
18.156022	916.238245	14.176935
18.125220	917.035114	14.181952
18.414402	916.371182	14.186970
18.276887	915.408025	14.191987
18.263398	914.059356	14.197005
18.605907	910.168098	14.202023
18.258886	911.734047	14.207040
18.255804	915.429958	14.212058
18.634442	912.148430	14.217075
18.401978	912.393062	14.222093
18.357959	915.906037	14.227111
17.977483	923.053623	14.232128
18.261788	929.364896	14.237146
18.535249	938.559168	14.242163
18.599246	943.361749	14.247181
18.546310	934.577746	14.252199
18.518002	942.781024	14.257216
18.657193	950.197501	14.262234
18.774329	937.618753	14.267251
18.700691	936.045973	14.272269
18.674767	945.678483	14.277287
18.846975	944.332276	14.282304
18.902592	947.302617	14.287322
18.734316	939.480285	14.292339
18.429499	942.541812	14.297357
18.718468	934.183930	14.302375
18.737481	938.990402	14.307392
18.963694	939.257845	14.312410
18.506039	936.217798	14.317427
18.896864	941.474109	14.322445
18.688590	940.563063	14.327463
18.607684	941.774889	14.332480
19.059952	948.725739	14.337498
18.719758	942.192686	14.342515
18.748003	946.486464	14.347533
18.633364	946.782065	14.352551
19.322385	954.835088	14.357568
19.373629	947.107748	14.362586
19.358119	941.467426	14.367603
19.176291	935.531267	14.372621
19.233968	936.734003	14.377639
18.987147	943.469330	14.382656
19.255841	936.771450	14.387674
19.049008	935.970633	14.392691
19.156797	936.101994	14.397709
19.072404	935.954192	14.402727
19.244334	936.018697	14.407744
19.421043	934.002744	14.412762
19.255615	927.107793	14.417779
18.931946	928.979358	14.422797
19.415656	926.684928	14.427815
19.232498	928.752232	14.432832
19.452409	931.365464	14.437850
19.222973	930.255759	14.442867
19.058438	933.967503	14.447885
19.466439	926.455680	14.452903
19.210380	934.356962	14.457920
19.560321	930.562366	14.462938
19.673719	932.299179	14.467955
19.339236	931.221713	14.472973
19.486055	932.145390	14.477991
19.345205	940.202196	14.483008
19.286878	930.873076	14.488026
19.559136	929.656364	14.493043
19.477330	928.605581	14.498061
19.642557	926.477817	14.503079
19.355048	930.391867	14.508096
19.512498	929.713859	14.513114
19.472014	931.496873	14.518131
19.519433	946.804748	14.523149
19.695387	953.994555	14.528167
19.548041	954.954856	14.533184
19.788375	957.965686	14.538202
19.617956	965.967175	14.543219
19.883817	963.441780	14.548237
19.925639	958.530941	14.553255
19.476407	952.317931	14.558272
19.920092	963.618908	14.563290
19.873568	950.769141	14.568307
19.630568	947.723863	14.573325
19.477541	954.917877	14.578343
19.766610	963.885651	14.583360
19.604332	969.493722	14.588378
20.020444	963.498583	14.593395
19.605913	964.172537	14.598413
19.840936	963.914727	14.603431
19.898046	960.696191	14.608448
19.675358	955.063078	14.613466
19.712006	950.670613	14.618483
19.450902	956.694959	14.623501
19.756741	960.544453	14.628519
20.021549	969.954696	14.633536
19.966826	980.342832	14.638554
20.284742	972.860883	14.643571
20.374964	969.662404	14.648589
20.330598	956.345228	14.653607
19.676974	948.838781	14.658624
19.830619	960.257784	14.663642
19.968052	978.672730	14.668659
20.019003	986.062020	14.673677
20.508322	984.950153	14.678695
20.188203	986.982117	14.683712
20.465457	980.263944	14.688730
20.514023	985.371918	14.693747
20.043151	979.484187	14.698765
20.173404	969.093532	14.703783
20.011102	980.732466	14.708800
20.205998	983.800914	14.713818
20.532651	976.156646	14.718835
20.552537	982.424158	14.723853
20.166701	978.271454	14.728871
20.134213	976.670133	14.733888
20.166190	969.867315	14.738906
20.389651	973.291054	14.743923
20.415700	980.053070	14.748941
20.584631	972.013785	14.753959
20.755495	979.128660	14.758976
20.496872	979.759251	14.763994
20.751977	972.249274	14.769011
20.519931	976.356619	14.774029
20.587198	967.140348	14.779047
20.593518	974.041156	14.784064
20.577711	974.337052	14.789082
20.528362	971.412910	14.794099
20.514056	973.835623	14.799117
20.694551	979.850748	14.804135
20.968632	976.702357	14.809152
20.600093	969.580432	14.814170
20.410656	973.946194	14.819187
20.568493	974.205416	14.824205
20.823857	971.306116	14.829223
20.744417	978.772639	14.834240
20.433158	976.334509	14.839258
20.693922	968.618515	14.844275
20.680825	976.743685	14.849293
20.827145	994.481900	14.854311
21.171359	997.233459	14.859328
20.814922	992.618544	14.864346
20.977648	982.459484	14.869363
21.040312	994.631236	14.874381
21.030263	990.249234	14.879399
20.999451	974.184316	14.884416
20.852942	984.795123	14.889434
21.474735	984.145348	14.894451
21.151276	977.682245	14.899469
20.892195	972.818548	14.904487
21.045793	964.459770	14.909504
20.932902	968.308599	14.914522
20.943198	984.995123	14.919539
21.211985	999.700303	14.924557
20.863426	1002.408925	14.929575
21.016026	998.610520	14.934592
20.918464	996.164152	14.939610
21.227208	996.346081	14.944627
21.251802	997.897994	14.949645
21.425593	996.166519	14.954663
21.126856	994.966681	14.959680
21.060055	998.309668	14.964698
21.462797	991.066891	14.969715
20.792256	989.821163	14.974733
21.399624	997.934337	14.979751
21.508911	999.772789	14.984768
21.014484	1006.584805	14.989786
21.232385	995.060068	14.994803
21.181011	1011.784683	14.999821
21.555834	1018.495224	15.004839
21.637951	1023.175064	15.009856
21.980762	1016.768505	15.014874
21.763649	1005.965185	15.019891
21.260706	1002.241087	15.024909
21.588617	1017.725985	15.029927
21.807136	1018.856188	15.034944
21.818159	1005.665999	15.039962
21.747766	990.550874	15.044979
21.447842	994.927640	15.049997
21.522743	990.532328	15.055015
21.679783	998.798112	15.060032
22.082125	1005.608481	15.065050
22.112443	997.635084	15.070067
21.832963	992.963930	15.075085
21.694817	986.847336	15.080103
21.867530	977.444122	15.085120
21.863013	985.930876	15.090138
21.795195	981.905073	15.095155
21.863832	994.312579	15.100173
21.663085	987.104396	15.105191
22.114037	988.794639	15.110208
21.816993	986.130213	15.115226
22.036765	1001.209155	15.120243
21.888274	1003.387803	15.125261
22.022495	1018.398110	15.130279
22.050118	1010.687067	15.135296
22.154346	1014.097937	15.140314
22.076225	1000.975368	15.145331
22.020803	997.373661	15.150349
22.165123	1006.932193	15.155367
22.335459	998.438231	15.160384
22.053765	991.782382	15.165402
22.068530	989.700275	15.170419
22.016018	991.605103	15.175437
22.416986	1005.222894	15.180455
22.420872	1004.171305	15.185472
22.243177	998.297594	15.190490
22.210016	986.288325	15.195507
22.000974	987.548634	15.200525
22.223152	1004.012626	15.205543
22.563874	999.222206	15.210560
22.398239	1006.411905	15.215578
22.600383	1003.325275	15.220595
22.664093	995.027905	15.225613
22.021202	997.665874	15.230631
22.682773	1001.024132	15.235648
22.315390	1005.474587	15.240666
22.468075	1009.202918	15.245683
22.752761	1007.072207	15.250701
22.554954	1011.505563	15.255719
22.455593	1003.893316	15.260736
22.398205	1006.146054	15.265754
22.498010	1009.213626	15.270771
22.400918	1004.542295	15.275789
22.560930	1003.232709	15.280807
22.369883	1000.557986	15.285824
22.477659	1010.122245	15.290842
22.420671	1008.370121	15.295859
22.231823	1008.560583	15.300877
21.928472	1008.251422	15.305895
22.368741	1025.754260	15.310912
22.361153	1032.477385	15.315930
22.450078	1030.591942	15.320947
22.679432	1028.432027	15.325965
22.482782	1029.911308	15.330983
22.591375	1027.369519	15.336000
23.181165	1051.204886	15.341018
22.849487	1043.010469	15.346035
22.993215	1048.838870	15.351053
22.962782	1046.331483	15.356071
23.053780	1035.173751	15.361088
23.112466	1039.917228	15.366106
23.166996	1039.296369	15.371123
23.214067	1034.574039	15.376141
22.979191	1029.160568	15.381159
23.147549	1021.418002	15.386176
23.116645	1014.937451	15.391194
23.227963	1014.427617	15.396211
23.324139	1011.931957	15.401229
23.105443	1012.411124	15.406247
23.415788	1012.816869	15.411264
23.237085	1026.052118	15.416282
23.019585	1021.361777	15.421299
23.140397	1030.924004	15.426317
23.227987	1036.199451	15.431335
23.560761	1034.913289	15.436352
23.500804	1046.151214	15.441370
23.543380	1031.614814	15.446387
23.318835	1015.154170	15.451405
23.103212	1028.720261	15.456423
23.516037	1026.963955	15.461440
23.494557	1037.750868	15.466458
23.656173	1039.218199	15.471475
23.857964	1036.197892	15.476493
23.575442	1031.621880	15.481511
23.796167	1014.027943	15.486528
23.213112	1023.921359	15.491546
23.340485	1022.500119	15.496563
23.638074	1032.391263	15.501581
23.307084	1037.135832	15.506599
23.776608	1043.575920	15.511616
23.694925	1046.763454	15.516634
23.666513	1041.282915	15.521651
24.049612	1042.138020	15.526669
23.716257	1043.919594	15.531687
23.612778	1042.616574	15.536704
23.777056	1041.965895	15.541722
23.683869	1045.937889	15.546739
23.733746	1038.810340	15.551757
23.582114	1047.055080	15.556775
23.531260	1040.085328	15.561792
23.905046	1043.324579	15.566810
24.363056	1034.116481	15.571827
24.110526	1049.263151	15.576845
23.934905	1047.573794	15.581863
24.125037	1041.374188	15.586880
24.029944	1046.593052	15.591898
23.677439	1042.438266	15.596915
23.876923	1041.255040	15.601933
23.468667	1053.506927	15.606951
23.905263	1047.805204	15.611968
23.681493	1053.514456	15.616986
23.864486	1068.857999	15.622003
24.131182	1066.812153	15.627021
23.910565	1076.686681	15.632039
24.476281	1067.474315	15.637056
24.341968	1066.722092	15.642074
24.487000	1075.930246	15.647091
24.752898	1064.580986	15.652109
24.295763	1066.031653	15.657127
24.381534	1070.029263	15.662144
24.569565	1077.434984	15.667162
24.250498	1083.547351	15.672179
24.742679	1065.620491	15.677197
24.613378	1070.443924	15.682215
24.686930	1053.791369	15.687232
24.453521	1044.158253	15.692250
24.260768	1046.599467	15.697267
24.369912	1052.575303	15.702285
24.614850	1062.632507	15.707303
24.540685	1071.086032	15.712320
24.501853	1066.784262	15.717338
24.335050	1072.033304	15.722355
24.572314	1063.673995	15.727373
24.551898	1072.759743	15.732391
24.746869	1067.354653	15.737408
25.288050	1074.307401	15.742426
24.745695	1074.594277	15.747443
24.633320	1066.081460	15.752461
24.464533	1066.963073	15.757479
24.776829	1069.880595	15.762496
24.723473	1068.557096	15.767514
24.369491	1069.063772	15.772531
24.459063	1071.871020	15.777549
24.738658	1070.952958	15.782567
24.749801	1077.184003	15.787584
24.755663	1079.231176	15.792602
24.424370	1086.715113	15.797619
24.823816	1088.003170	15.802637
24.727171	1093.547347	15.807655
24.844146	1090.272069	15.812672
24.733098	1079.960183	15.817690
24.650058	1092.700799	15.822707
25.149789	1101.345295	15.827725
25.114481	1099.826457	15.832743
25.355782	1102.843473	15.837760
25.617932	1099.633813	15.842778
25.454883	1094.168041	15.847795
25.137387	1077.261144	15.852813
25.163155	1074.328371	15.857831
25.069510	1073.872741	15.862848
25.815890	1086.287735	15.867866
25.326647	1087.838111	15.872883
25.402805	1080.289851	15.877901
25.189577	1080.727136	15.882919
24.886582	1094.654113	15.887936
25.288156	1092.113748	15.892954
25.171386	1110.126834	15.897971
25.660642	1109.381054	15.902989
25.378105	1111.880526	15.908007
25.357847	1104.195881	15.913024
25.670805	1097.033402	15.918042
25.549005	1102.881332	15.923059
25.729129	1109.862261	15.928077
26.103959	1105.893311	15.933095
25.808092	1101.287813	15.938112
26.018918	1088.751085	15.943130
25.736257	1098.550138	15.948147
25.654848	1091.787130	15.953165
25.536001	1088.523554	15.958183
25.630671	1092.889014	15.963200
26.160834	1098.802055	15.968218
25.758353	1099.281616	15.973235
25.970496	1103.985288	15.978253
26.229646	1099.513743	15.983271
26.031259	1095.909169	15.988288
25.956406	1099.966667	15.993306
25.936296	1101.175290	15.998323
26.094777	1092.462229	16.003341
25.688569	1093.557771	16.008359
25.629516	1095.507817	16.013376
25.963738	1085.990876	16.018394
25.786024	1102.160999	16.023411
26.066428	1088.944321	16.028429
25.922449	1094.701047	16.033447
25.690456	1092.490329	16.038464
26.164964	1107.567319	16.043482
26.195707	1107.720220	16.048499
26.298908	1108.060590	16.053517
26.302042	1117.060618	16.058535
26.272948	1119.782321	16.063552
26.530535	1118.009303	16.068570
26.249581	1121.827691	16.073587
26.492747	1118.766173	16.078605
26.589418	1115.071183	16.083623
26.616817	1115.287726	16.088640
26.857644	1114.126421	16.093658
26.751945	1103.371859	16.098675
26.376617	1092.283998	16.103693
26.440929	1083.853945	16.108711
26.194349	1079.616281	16.113728
26.695076	1093.543566	16.118746
26.514287	1111.159574	16.123763
26.597187	1112.995860	16.128781
26.678973	1109.151721	16.133799
26.289130	1113.630969	16.138816
26.639541	1118.540205	16.143834
26.613179	1115.154833	16.148851
26.702824	1109.270758	16.153869
26.875587	1110.247186	16.158887
26.672269	1114.795043	16.163904
27.091023	1106.539826	16.168922
26.600865	1113.332278	16.173939
26.715664	1107.144453	16.178957
26.701660	1100.629663	16.183975
26.673162	1106.431417	16.188992
26.798318	1108.381005	16.194010
26.688139	1107.653402	16.199027
26.801607	1107.121138	16.204045
26.801030	1108.796929	16.209063
27.235394	1128.090182	16.214080
27.566995	1124.677127	16.219098
27.085262	1122.524469	16.224115
27.168618	1113.832635	16.229133
27.197098	1106.118261	16.234151
27.219432	1112.618971	16.239168
27.187518	1101.534105	16.244186
27.518796	1119.281336	16.249203
27.626335	1107.101614	16.254221
27.447662	1099.113579	16.259239
27.151024	1107.371598	16.264256
27.069330	1102.672581	16.269274
27.316840	1108.020826	16.274291
27.595322	1117.457408	16.279309
27.576269	1101.807110	16.284327
27.355591	1106.452361	16.289344
27.627876	1101.571648	16.294362
27.161323	1110.304427	16.299379
27.559109	1115.777455	16.304397
27.799279	1126.618104	16.309415
27.545154	1132.764494	16.314432
27.840394	1125.355465	16.319450
27.840835	1126.920641	16.324467
27.502811	1108.748262	16.329485
27.625172	1115.646723	16.334503
27.400192	1120.349457	16.339520
27.518466	1135.422324	16.344538
27.416153	1129.006569	16.349555
27.385252	1125.937496	16.354573
27.965076	1132.338243	16.359591
27.655754	1132.626479	16.364608
27.593695	1130.114568	16.369626
27.857480	1129.625026	16.374643
27.791292	1127.464066	16.379661
27.943798	1138.826556	16.384679
27.869540	1153.872797	16.389696
28.130112	1147.204514	16.394714
27.935580	1155.118345	16.399731
28.053142	1149.605434	16.404749
28.453799	1151.477147	16.409767
28.243568	1153.820126	16.414784
28.215443	1140.926313	16.419802
28.415982	1144.479912	16.424819
28.121085	1139.422959	16.429837
28.172870	1133.822527	16.434855
28.243572	1138.472627	16.439872
28.434523	1144.107463	16.444890
28.467586	1153.513086	16.449907
28.289827	1139.206786	16.454925
28.378331	1137.744288	16.459943
28.494766	1147.947911	16.464960
28.762646	1143.118371	16.469978
28.435985	1131.066625	16.474995
28.048983	1118.102821	16.480013
28.476491	1138.290276	16.485031
28.340098	1145.112522	16.490048
28.457272	1138.665530	16.495066
28.877378	1151.434656	16.500083
28.586442	1147.001948	16.505101
28.655106	1144.829325	16.510119
28.349035	1142.245188	16.515136
28.731091	1138.152019	16.520154
28.553521	1142.061514	16.525171
28.545419	1139.768372	16.530189
28.484690	1141.220054	16.535207
28.241510	1145.562719	16.540224
28.347816	1140.764807	16.545242
28.690577	1157.989555	16.550259
28.865368	1173.934094	16.555277
28.801057	1167.376668	16.560295
28.809596	1184.372931	16.565312
28.898631	1173.086028	16.570330
28.712188	1175.292735	16.575347
29.108560	1177.616416	16.580365
29.269232	1168.587384	16.585383
29.006101	1174.792006	16.590400
29.136171	1168.197813	16.595418
29.098852	1174.546941	16.600435
28.755556	1170.974523	16.605453
29.081792	1174.022426	16.610471
28.947479	1168.990799	16.615488
28.988108	1168.394204	16.620506
29.258898	1185.100063	16.625523
29.087403	1199.722908	16.630541
29.564262	1194.302017	16.635559
29.289576	1196.475213	16.640576
29.553298	1193.552478	16.645594
29.570974	1196.547740	16.650611
29.663461	1202.507300	16.655629
29.680045	1193.582885	16.660647
29.832846	1193.883926	16.665664
29.597441	1182.887698	16.670682
29.787273	1175.589840	16.675699
29.596500	1178.548329	16.680717
29.798809	1162.752839	16.685735
29.377243	1166.126194	16.690752
29.828980	1173.976647	16.695770
29.616930	1184.869249	16.700787
29.699834	1192.256774	16.705805
29.839473	1184.903659	16.710823
29.720451	1189.892776	16.715840
29.671384	1184.689994	16.720858
29.740457	1193.237902	16.725875
29.875698	1188.485939	16.730893
29.783294	1182.977512	16.735911
29.566490	1194.615657	16.740928
29.859598	1190.410177	16.745946
30.111258	1185.542140	16.750963
29.693100	1188.081808	16.755981
29.896840	1184.168050	16.760999
29.756233	1193.859689	16.766016
30.100294	1203.576385	16.771034
30.357541	1205.912400	16.776051
30.028934	1213.348630	16.781069
30.339658	1205.754099	16.786087
30.364992	1218.436797	16.791104
30.469380	1215.551646	16.796122
30.011655	1205.331875	16.801139
30.435721	1224.718368	16.806157
30.364030	1211.765055	16.811175
30.418259	1217.519169	16.816192
30.306918	1211.846437	16.821210
30.512075	1210.229952	16.826227
30.537679	1220.236401	16.831245
30.512861	1211.839189	16.836263
30.630453	1204.558949	16.841280
30.624818	1204.597626	16.846298
30.921073	1204.358623	16.851315
30.581789	1209.852487	16.856333
30.430011	1197.221012	16.861351
30.191371	1208.079923	16.866368
30.636894	1198.659096	16.871386
30.949158	1199.739909	16.876403
30.425380	1206.648120	16.881421
30.615456	1196.727657	16.886439
30.624278	1206.960798	16.891456
30.750612	1208.695611	16.896474
30.394630	1209.546598	16.901491
30.562360	1213.544023	16.906509
31.079037	1220.598501	16.911527
30.949673	1237.935169	16.916544
31.156141	1227.500864	16.921562
30.963036	1223.153797	16.926579
31.013553	1230.562192	16.931597
31.122054	1228.856705	16.936615
31.028647	1234.542433	16.941632
31.157978	1225.369956	16.946650
31.514658	1239.985822	16.951667
31.589357	1231.942249	16.956685
31.533847	1230.647479	16.961703
31.369375	1239.342459	16.966720
31.091250	1229.795146	16.971738
31.279354	1228.307568	16.976755
31.300209	1227.938139	16.981773
31.673461	1229.283962	16.986791
31.540756	1232.785646	16.991808
31.103245	1236.625431	16.996826
31.462169	1235.426680	17.001843
31.294582	1237.955498	17.006861
31.467469	1234.633563	17.011879
31.242651	1230.667017	17.016896
31.285830	1223.903374	17.021914
31.667988	1216.840462	17.026931
31.312444	1229.847940	17.031949
31.426006	1228.918014	17.036967
31.719290	1239.538963	17.041984
31.745510	1245.108119	17.047002
31.982541	1245.995588	17.052019
31.929674	1254.161830	17.057037
31.973748	1245.179432	17.062055
31.954005	1256.124000	17.067072
31.827648	1251.630764	17.072090
32.579439	1249.429996	17.077107
31.925672	1254.092646	17.082125
31.967816	1235.507111	17.087143
31.998956	1247.690287	17.092160
31.729692	1245.851474	17.097178
32.226837	1247.313592	17.102195
32.139609	1254.532132	17.107213
32.237029	1251.695406	17.112231
31.918074	1243.666166	17.117248
31.775486	1242.571237	17.122266
32.331818	1240.846078	17.127283
32.071060	1241.868345	17.132301
32.129785	1244.617335	17.137319
32.390867	1243.563305	17.142336
32.239331	1249.466436	17.147354
32.505668	1254.786528	17.152371
32.809433	1260.476311	17.157389
32.273681	1248.794928	17.162407
32.527396	1250.935836	17.167424
32.463184	1273.456965	17.172442
32.864657	1267.946874	17.177459
32.583078	1266.157327	17.182477
32.413392	1266.259579	17.187495
32.496440	1267.161707	17.192512
32.627886	1270.429501	17.197530
32.836939	1270.002181	17.202547
32.571104	1274.979610	17.207565
32.624513	1267.630503	17.212583
33.056619	1268.171817	17.217600
32.713284	1267.228264	17.222618
33.307072	1268.599499	17.227635
32.803436	1276.031619	17.232653
32.613294	1274.514934	17.237671
32.853405	1268.818678	17.242688
32.579252	1273.762695	17.247706
32.751931	1271.712621	17.252723
33.449422	1277.463802	17.257741
32.783781	1277.656382	17.262759
32.856840	1273.535854	17.267776
33.357592	1285.525553	17.272794
33.473763	1290.067580	17.277811
33.345392	1278.060408	17.282829
33.157171	1280.182196	17.287847
33.261414	1284.644036	17.292864
32.984040	1291.968126	17.297882
33.446186	1285.217715	17.302899
33.059525	1291.637398	17.307917
32.973560	1290.773445	17.312935
33.237815	1281.668165	17.317952
33.342398	1293.357009	17.322970
33.680095	1284.398017	17.327987
33.438188	1288.532226	17.333005
33.591377	1283.363999	17.338023
33.561318	1285.662986	17.343040
33.685727	1290.610835	17.348058
34.037266	1295.002373	17.353075
33.666455	1292.586153	17.358093
33.529760	1294.235949	17.363111
33.894570	1295.377965	17.368128
33.918495	1311.734443	17.373146
34.258531	1304.084783	17.378163
34.246446	1308.261886	17.383181
33.953185	1293.929376	17.388199
34.043969	1285.346753	17.393216
34.028027	1285.910928	17.398234
34.084163	1281.657345	17.403251
33.732183	1288.380874	17.408269
34.459728	1295.153026	17.413287
34.165652	1304.035606	17.418304
34.110017	1305.981984	17.423322
34.415889	1302.973728	17.428339
34.186060	1308.810248	17.433357
34.245960	1310.918411	17.438375
34.487423	1296.536835	17.443392
33.946438	1302.365297	17.448410
34.207237	1301.456480	17.453427
34.511944	1305.268357	17.458445
34.725703	1299.920216	17.463463
34.986143	1297.594447	17.468480
34.568625	1306.524772	17.473498
34.918425	1294.736172	17.478515
34.572810	1294.711347	17.483533
34.379659	1298.143617	17.488551
34.731361	1294.945139	17.493568
34.895783	1300.650455	17.498586
34.937250	1302.013552	17.503603
34.521703	1306.146567	17.508621
34.717606	1303.600527	17.513639
34.797512	1295.830675	17.518656
34.587821	1299.215041	17.523674
34.497508	1304.480570	17.528691
34.618153	1299.648810	17.533709
34.469307	1293.114049	17.538727
34.567703	1298.157498	17.543744
34.507125	1305.075227	17.548762
34.933823	1319.004821	17.553779
34.670338	1333.809452	17.558797
34.727104	1323.379610	17.563815
35.087329	1319.807393	17.568832
34.672504	1334.250713	17.573850
34.777891	1337.279596	17.578867
35.191185	1343.826437	17.583885
35.040254	1346.163305	17.588903
35.219274	1351.525510	17.593920
35.315566	1342.399176	17.598938
35.327631	1351.274842	17.603955
35.289309	1353.000752	17.608973
35.261641	1353.936010	17.613991
35.404804	1349.160671	17.619008
35.383542	1355.876592	17.624026
35.919580	1347.744906	17.629043
35.833239	1343.785042	17.634061
35.740878	1347.375105	17.639079
35.980316	1343.244273	17.644096
35.924645	1346.970605	17.649114
36.041593	1337.566471	17.654131
35.559724	1341.839279	17.659149
35.776016	1353.441230	17.664167
35.854036	1341.108177	17.669184
35.821609	1348.356041	17.674202
35.932236	1344.753495	17.679219
35.701398	1347.260679	17.684237
35.873267	1360.087784	17.689255
35.989183	1347.404793	17.694272
35.758076	1348.952617	17.699290
35.803187	1341.317590	17.704307
35.909284	1345.280518	17.709325
35.696386	1364.479771	17.714343
36.066870	1358.557925	17.719360
35.917756	1362.387266	17.724378
35.637421	1361.948255	17.729395
36.115961	1368.156665	17.734413
35.968497	1369.113850	17.739431
36.578944	1377.794785	17.744448
36.434902	1393.278213	17.749466
36.585529	1383.408012	17.754483
36.709984	1389.122774	17.759501
36.250853	1374.629987	17.764519
36.554318	1380.932107	17.769536
36.653841	1381.588652	17.774554
36.637487	1385.539215	17.779571
37.078591	1381.780738	17.784589
37.195979	1387.954218	17.789607
36.866950	1375.905832	17.794624
36.733088	1369.532805	17.799642
36.705832	1368.574439	17.804659
36.688868	1367.336739	17.809677
36.828922	1380.749535	17.814695
37.400924	1387.037987	17.819712
37.152256	1373.055047	17.824730
36.916816	1370.017979	17.829747
37.165444	1361.615724	17.834765
37.020289	1360.518034	17.839783
36.822445	1359.223464	17.844800
37.052860	1370.791654	17.849818
37.240240	1381.022166	17.854835
37.312510	1377.627603	17.859853
36.932982	1391.137593	17.864871
37.448843	1386.395373	17.869888
37.231943	1387.524391	17.874906
37.252370	1385.018456	17.879923
37.433905	1373.814768	17.884941
37.385168	1386.111542	17.889959
37.744358	1371.796671	17.894976
37.480550	1372.920413	17.899994
37.421503	1388.100173	17.905011
37.507535	1376.842016	17.910029
37.429287	1384.901837	17.915047
37.606228	1385.236971	17.920064
37.632337	1391.885520	17.925082
37.421506	1391.132648	17.930099
37.771764	1375.446339	17.935117
37.460300	1384.259097	17.940135
37.747949	1383.516491	17.945152
37.683968	1382.917343	17.950170
37.424102	1395.818428	17.955187
37.773563	1394.548563	17.960205
37.764041	1417.534695	17.965223
37.817472	1409.929894	17.970240
37.789226	1401.763513	17.975258
37.811794	1415.065349	17.980275
37.723422	1413.453808	17.985293
37.694543	1413.818034	17.990311
37.681710	1417.566072	17.995328
38.203498	1432.178319	18.000346
38.171679	1433.294121	18.005363
38.283161	1422.855649	18.010381
38.281833	1438.856422	18.015399
38.356668	1434.820790	18.020416
39.024886	1434.618185	18.025434
38.895110	1434.815174	18.030451
38.908525	1427.314470	18.035469
38.708586	1428.071587	18.040487
38.116344	1429.960034	18.045504
38.318039	1433.573474	18.050522
38.343256	1433.029780	18.055539
38.134709	1425.999374	18.060557
38.193979	1437.704880	18.065575
38.773166	1428.136754	18.070592
39.046598	1432.108199	18.075610
38.628173	1428.730545	18.080627
38.949291	1440.767429	18.085645
38.723827	1456.667629	18.090663
38.884810	1450.453515	18.095680
39.025391	1445.931030	18.100698
39.263512	1452.779925	18.105715
39.573518	1444.298585	18.110733
39.153137	1450.600526	18.115751
39.295062	1446.598562	18.120768
39.553202	1439.053199	18.125786
38.932321	1431.323655	18.130803
39.325746	1424.410382	18.135821
39.501271	1435.703180	18.140839
39.706412	1429.864023	18.145856
39.164565	1417.937319	18.150874
39.225300	1418.593631	18.155891
39.646816	1423.034200	18.160909
39.259133	1437.457571	18.165927
39.515129	1432.705558	18.170944
39.726212	1438.277370	18.175962
39.849869	1442.174450	18.180979
39.592260	1430.039095	18.185997
39.793472	1430.348336	18.191015
39.826828	1433.189696	18.196032
39.480047	1440.606775	18.201050
39.611347	1434.132216	18.206067
40.160359	1427.219813	18.211085
40.025660	1431.491899	18.216103
39.753313	1436.009624	18.221120
39.519670	1446.467091	18.226138
39.636429	1445.779661	18.231155
39.884025	1432.823502	18.236173
39.669811	1442.037636	18.241191
39.786305	1441.239789	18.246208
40.062632	1452.033944	18.251226
39.959852	1470.900463	18.256243
40.310869	1464.606074	18.261261
40.086662	1467.304749	18.266279
39.950621	1464.858033	18.271296
39.926566	1470.532971	18.276314
39.928759	1473.508614	18.281331
40.485735	1460.500807	18.286349
40.543177	1466.459634	18.291367
40.232164	1473.293583	18.296384
40.251052	1469.165718	18.301402
40.286943	1483.393367	18.306419
40.946772	1481.175421	18.311437
40.524234	1490.075064	18.316455
40.839002	1490.669486	18.321472
40.637175	1490.281290	18.326490
40.626527	1494.145771	18.331507
40.964548	1489.696489	18.336525
40.696418	1493.042708	18.341543
40.908580	1489.834499	18.346560
40.992720	1490.272542	18.351578
40.896371	1486.017554	18.356595
40.960066	1492.508766	18.361613
40.895591	1494.178824	18.366631
40.888341	1491.036552	18.371648
41.378570	1490.135964	18.376666
40.632687	1495.598939	18.381683
40.930404	1489.262398	18.386701
41.412546	1492.140755	18.391719
41.073348	1495.927320	18.396736
41.432293	1506.052124	18.401754
40.926622	1514.731263	18.406771
41.447726	1501.877377	18.411789
41.229954	1516.280501	18.416807
41.282382	1510.256952	18.421824
41.638945	1514.458400	18.426842
41.249095	1520.812389	18.431859
41.462449	1507.741615	18.436877
41.351981	1515.055424	18.441895
41.415792	1511.911482	18.446912
41.564039	1527.753194	18.451930
41.743104	1542.655926	18.456947
41.951808	1524.993940	18.461965
41.997906	1534.621795	18.466983
42.080072	1534.946533	18.472000
42.337926	1532.684259	18.477018
41.877441	1531.131009	18.482035
42.237809	1536.060893	18.487053
42.227347	1530.151337	18.492071
42.065630	1530.539534	18.497088
42.358686	1527.331268	18.502106
42.272249	1523.554425	18.507123
41.951796	1525.753766	18.512141
42.243489	1526.124575	18.517159
42.197226	1522.145767	18.522176
42.200216	1521.176343	18.527194
42.274710	1521.458099	18.532211
42.319444	1517.572339	18.537229
42.642346	1524.985519	18.542247
42.497632	1522.997768	18.547264
42.576580	1516.509291	18.552282
42.636735	1524.525399	18.557299
42.554047	1522.868774	18.562317
42.461214	1522.267830	18.567335
42.047951	1522.869016	18.572352
42.533361	1529.688664	18.577370
42.723161	1542.784504	18.582387
43.039122	1554.251043	18.587405
42.960280	1551.312491	18.592423
42.671259	1558.606953	18.597440
43.161289	1551.063083	18.602458
42.819067	1558.968671	18.607475
43.103511	1549.263614	18.612493
43.221572	1545.334799	18.617511
43.041897	1554.067028	18.622528
42.981739	1544.750498	18.627546
42.932761	1557.956346	18.632563
43.024070	1544.910979	18.637581
42.971257	1540.567102	18.642599
42.841762	1561.782784	18.647616
43.092739	1572.208579	18.652634
42.845244	1576.381601	18.657651
42.943628	1579.534705	18.662669
43.438364	1571.983777	18.667687
43.509843	1583.425520	18.672704
43.918099	1580.852482	18.677722
43.598671	1585.696374	18.682739
43.752215	1586.032022	18.687757
43.909450	1589.030732	18.692775
43.767677	1603.172697	18.697792
44.035280	1582.698920	18.702810
43.992877	1594.079614	18.707827
43.945831	1594.443533	18.712845
44.107546	1587.626466	18.717863
43.923207	1596.709759	18.722880
44.245011	1588.800889	18.727898
44.360344	1598.449491	18.732915
44.309868	1586.653982	18.737933
44.139074	1578.049082	18.742951
44.108315	1581.317099	18.747968
44.397529	1584.516049	18.752986
44.474850	1578.718962	18.758003
44.410309	1590.989950	18.763021
44.547221	1584.198862	18.768039
44.377262	1588.028361	18.773056
44.590988	1579.776647	18.778074
44.380026	1581.835757	18.783091
44.731816	1581.919427	18.788109
44.740726	1582.574397	18.793127
44.102411	1589.159853	18.798144
44.502837	1586.859454	18.803162
44.278201	1586.560040	18.808179
44.179183	1581.443867	18.813197
44.766526	1590.008600	18.818215
44.599823	1603.141404	18.823232
44.815556	1602.845581	18.828250
44.729907	1611.597822	18.833267
44.808565	1615.520926	18.838285
44.882411	1613.041305	18.843303
44.976222	1616.794768	18.848320
45.030726	1605.550875	18.853338
45.154490	1607.103083	18.858355
45.016555	1609.933437	18.863373
45.377396	1607.304705	18.868391
45.090393	1625.515403	18.873408
45.212961	1629.674641	18.878426
45.449873	1640.664444	18.883443
45.452469	1640.269463	18.888461
45.474088	1628.970744	18.893479
45.315839	1630.538736	18.898496
45.687747	1635.911833	18.903514
45.426170	1632.550592	18.908531
45.256862	1631.658652	18.913549
45.793113	1627.645363	18.918567
45.631646	1628.595287	18.923584
45.881580	1632.993360	18.928602
45.679079	1628.171113	18.933619
45.659473	1633.069034	18.938637
45.626890	1631.221502	18.943655
46.160141	1639.835762	18.948672
46.077168	1652.425278	18.953690
46.104351	1651.584607	18.958707
45.933726	1647.341218	18.963725
46.368430	1654.929451	18.968743
46.306564	1649.883181	18.973760
46.545503	1650.625197	18.978778
46.352063	1649.907460	18.983795
46.067371	1648.105738	18.988813
46.462971	1649.482809	18.993831
46.132027	1647.644149	18.998848
46.313488	1646.009247	19.003866
46.426655	1645.246628	19.008883
46.396034	1646.740974	19.013901
46.683684	1641.961855	19.018919
46.633035	1647.180242	19.023936
46.922551	1647.005410	19.028954
46.815573	1647.545988	19.033971
46.757890	1648.025191	19.038989
46.737159	1643.632078	19.044007
46.709890	1653.381951	19.049024
47.012399	1646.028377	19.054042
47.271070	1657.746970	19.059059
46.668689	1665.967936	19.064077
47.051777	1665.443909	19.069095
46.957843	1669.390909	19.074112
47.234245	1671.935437	19.079130
47.486253	1673.256108	19.084147
47.508029	1674.467675	19.089165
47.498800	1665.663840	19.094183
47.472826	1675.176823	19.099200
47.472656	1669.199333	19.104218
47.434778	1665.973461	19.109235
47.186093	1675.079499	19.114253
47.231637	1674.276978	19.119271
46.982929	1658.210869	19.124288
47.069238	1675.687748	19.129306
47.573929	1675.605443	19.134323
47.569998	1693.178534	19.139341
47.440336	1694.420141	19.144359
47.454133	1700.903467	19.149376
47.122529	1697.815133	19.154394
47.647303	1694.753581	19.159411
47.545507	1714.210372	19.164429
47.741842	1715.101085	19.169447
48.076108	1717.545030	19.174464
48.119080	1710.774924	19.179482
48.103750	1712.462550	19.184499
48.073450	1717.804009	19.189517
48.254151	1707.004211	19.194535
48.219281	1713.362615	19.199552
47.968437	1722.083984	19.204570
48.262851	1713.399820	19.209587
48.280103	1724.727066	19.214605
48.615923	1738.598638	19.219623
48.671330	1740.085825	19.224640
48.632570	1739.476401	19.229658
49.005720	1732.547252	19.234675
48.844524	1737.865041	19.239693
49.023685	1730.363490	19.244711
48.666067	1716.889686	19.249728
48.719647	1713.482208	19.254746
49.006741	1720.295130	19.259763
48.829648	1736.247963	19.264781
49.328790	1730.173286	19.269799
49.072921	1729.279123	19.274816
49.126723	1721.364845	19.279834
49.227676	1714.686645	19.284851
48.854829	1731.029927	19.289869
49.203336	1724.016274	19.294887
49.128749	1732.227165	19.299904
48.834639	1737.499502	19.304922
49.191292	1732.147781	19.309939
49.025881	1727.515368	19.314957
49.224691	1724.741582	19.319975
49.215489	1737.682539	19.324992
49.178495	1736.321711	19.330010
49.825713	1755.326659	19.335027
49.544066	1759.394613	19.340045
50.041894	1753.386411	19.345063
49.638877	1758.041461	19.350080
49.573801	1761.763040	19.355098
49.903404	1747.891190	19.360115
49.360910	1751.305690	19.365133
49.627786	1752.819710	19.370151
49.838893	1756.015148	19.375168
49.883977	1761.691970	19.380186
50.165538	1756.705479	19.385203
50.019429	1772.243210	19.390221
49.928306	1779.326863	19.395239
50.401441	1779.962759	19.400256
50.214853	1778.783166	19.405274
50.774413	1779.474954	19.410291
50.512630	1775.444645	19.415309
50.437504	1776.182221	19.420327
50.533215	1779.774464	19.425344
50.261081	1778.706110	19.430362
50.750519	1775.590117	19.435379
50.468683	1768.277550	19.440397
50.633970	1770.571240	19.445415
50.747688	1774.911791	19.450432
50.477775	1775.812437	19.455450
50.983336	1767.808422	19.460467
50.749429	1773.210202	19.465485
51.340650	1765.296916	19.470503
51.125123	1768.562356	19.475520
50.897156	1777.046623	19.480538
50.814572	1770.258294	19.485555
50.523363	1781.905321	19.490573
51.169058	1789.220697	19.495591
51.053624	1788.714809	19.500608
51.019947	1792.901721	19.505626
51.447423	1795.735042	19.510643
51.250090	1794.030078	19.515661
51.270304	1790.031327	19.520679
51.384782	1795.842463	19.525696
51.326824	1798.578260	19.530714
51.657078	1789.396107	19.535731
51.041206	1801.488514	19.540749
51.527025	1805.827581	19.545767
51.789079	1811.861770	19.550784
51.672831	1822.815492	19.555802
51.815785	1822.972911	19.560819
52.063964	1819.781094	19.565837
52.037529	1811.620554	19.570855
52.016899	1812.579981	19.575872
51.905008	1819.950946	19.580890
52.011852	1819.444948	19.585907
52.057524	1817.534640	19.590925
51.939182	1812.159479	19.595943
52.012898	1814.858868	19.600960
52.021191	1815.681212	19.605978
52.330316	1822.897846	19.610995
52.541738	1833.377331	19.616013
52.597058	1848.078784	19.621031
52.618592	1840.371495	19.626048
52.689952	1847.997801	19.631066
52.733077	1841.991378	19.636083
52.603523	1841.298340	19.641101
52.766907	1843.983684	19.646119
52.868898	1845.277376	19.651136
52.749927	1839.877057	19.656154
53.134293	1825.065542	19.661171
52.822972	1836.321254	19.666189
53.191499	1845.920851	19.671207
53.026097	1846.606297	19.676224
53.083405	1836.813588	19.681242
52.946967	1837.920558	19.686259
52.773846	1850.410720	19.691277
52.724587	1852.630731	19.696295
52.790407	1842.057149	19.701312
52.821572	1841.376802	19.706330
53.202296	1853.085868	19.711347
53.388325	1859.210885	19.716365
53.333905	1860.854154	19.721383
53.185779	1866.315110	19.726400
53.612453	1864.777478	19.731418
53.732856	1860.453725	19.736435
53.638737	1870.962167	19.741453
53.307941	1869.016156	19.746471
53.582692	1878.299081	19.751488
53.731428	1892.114871	19.756506
53.711502	1883.546152	19.761523
53.883901	1889.360867	19.766541
53.767084	1887.132003	19.771559
53.879313	1882.269845	19.776576
53.851611	1885.619496	19.781594
54.251023	1889.877440	19.786611
54.252246	1883.893348	19.791629
53.937673	1896.093258	19.796647
54.400154	1901.171359	19.801664
54.357481	1909.882295	19.806682
54.435956	1906.701271	19.811699
54.247278	1897.938061	19.816717
54.575472	1911.053516	19.821735
54.872295	1900.349026	19.826752
54.665366	1899.661796	19.831770
55.033966	1897.154892	19.836787
54.709651	1907.033499	19.841805
54.786069	1909.034997	19.846823
55.270794	1899.339401	19.851840
55.054964	1903.201402	19.856858
55.014824	1892.098399	19.861875
55.069610	1896.968956	19.866893
54.652812	1897.103614	19.871911
55.017502	1890.021085	19.876928
54.677287	1898.144272	19.881946
55.196565	1908.253653	19.886963
55.585794	1914.504654	19.891981
55.238060	1924.197578	19.896999
55.409246	1916.627766	19.902016
55.384311	1912.304679	19.907034
55.289501	1922.055812	19.912051
55.715387	1919.325320	19.917069
55.433710	1928.351442	19.922087
55.537170	1917.519435	19.927104
55.497380	1919.397120	19.932122
55.550448	1917.015394	19.937139
55.467550	1933.720559	19.942157
55.695522	1944.023935	19.947175
55.944948	1949.678268	19.952192
56.005672	1945.663668	19.957210
56.393282	1953.445614	19.962227
56.075901	1943.468536	19.967245
56.322453	1955.085074	19.972263
56.031083	1944.381188	19.977280
56.173048	1946.094689	19.982298
56.132012	1947.256151	19.987315
56.203837	1946.903969	19.992333
56.339547	1946.806886	19.997351
56.139506	1944.736231	20.002368
56.384812	1962.693446	20.007386
56.193449	1967.845603	20.012403
56.580103	1970.486517	20.017421
56.508677	1976.216377	20.022439
56.720291	1966.017541	20.027456
56.925442	1972.379459	20.032474
56.989313	1964.851689	20.037491
57.055107	1963.096015	20.042509
56.799183	1968.488679	20.047527
56.679972	1962.921090	20.052544
56.687696	1977.917306	20.057562
57.255118	1987.290144	20.062579
57.353481	1991.570031	20.067597
57.132350	1992.137972	20.072615
57.501440	1988.658917	20.077632
57.462842	1994.563535	20.082650
57.631929	1990.980105	20.087667
57.700214	1984.669868	20.092685
57.532563	1992.838650	20.097703
58.217613	1987.321785	20.102720
58.073478	1981.799124	20.107738
57.775674	1984.171710	20.112755
57.804266	1986.928691	20.117773
57.856493	1983.240486	20.122791
57.987559	1978.113400	20.127808
57.586930	1979.239678	20.132826
57.899474	1978.568894	20.137843
58.017438	1981.479142	20.142861
57.670864	1989.271982	20.147879
58.343561	1993.928981	20.152896
58.448760	1998.643334	20.157914
58.420607	1997.763976	20.162931
58.729780	2004.049643	20.167949
58.321415	2003.119393	20.172967
58.499590	2009.147854	20.177984
58.768857	2007.615936	20.183002
58.750281	2011.734256	20.188019
59.066750	2013.688687	20.193037
58.723364	2011.681512	20.198055
59.036204	2007.002500	20.203072
58.662172	2008.579084	20.208090
58.830546	2005.355553	20.213107
58.590867	2000.908287	20.218125
58.316729	2004.466996	20.223143
59.001328	2005.628391	20.228160
58.954693	2025.468227	20.233178
58.884398	2030.857074	20.238195
59.264641	2031.583280	20.243213
59.036008	2040.525402	20.248231
59.380022	2022.444065	20.253248
59.286196	2031.292473	20.258266
59.123852	2028.843488	20.263283
59.431349	2026.516567	20.268301
59.453043	2022.978316	20.273319
59.754408	2027.785028	20.278336
59.875439	2033.541562	20.283354
59.420628	2045.346945	20.288371
59.767584	2040.192329	20.293389
59.708224	2047.649838	20.298407
59.834634	2041.365191	20.303424
59.948205	2043.872163	20.308442
59.521395	2045.201378	20.313459
59.780988	2047.202597	20.318477
59.683606	2048.628534	20.323495
60.190939	2060.428362	20.328512
60.109199	2062.631395	20.333530
60.405456	2068.679249	20.338547
60.912672	2051.859984	20.343565
60.421150	2066.764067	20.348583
60.386476	2063.534465	20.353600
60.381254	2061.035610	20.358618
60.100888	2056.739884	20.363635
60.684848	2064.904558	20.368653
60.874589	2077.940834	20.373671
61.121334	2086.193068	20.378688
60.858157	2084.277467	20.383706
60.815821	2092.953723	20.388723
61.034868	2084.571547	20.393741
60.925611	2096.067182	20.398759
61.178341	2081.661121	20.403776
61.367437	2087.227112	20.408794
61.069622	2079.778054	20.413811
60.922604	2089.209227	20.418829
61.082352	2085.715611	20.423847
61.028511	2085.553543	20.428864
61.321563	2109.771361	20.433882
61.342172	2115.243829	20.438899
61.647899	2105.134319	20.443917
62.081740	2121.790261	20.448935
61.858711	2118.448136	20.453952
61.803295	2104.551120	20.458970
61.779333	2111.318244	20.463987
62.013034	2101.415697	20.469005
61.425492	2109.359960	20.474023
61.910460	2109.684722	20.479040
61.982506	2123.427492	20.484058
62.137921	2127.960428	20.489075
62.437023	2128.753004	20.494093
62.603441	2132.653003	20.499111
62.471889	2133.165885	20.504128
62.668723	2114.921306	20.509146
62.181606	2125.920695	20.514163
62.689903	2121.056384	20.519181
62.721424	2130.996138	20.524199
62.684548	2121.483139	20.529216
62.680214	2121.483742	20.534234
62.804254	2131.484746	20.539251
62.998100	2124.346835	20.544269
62.970211	2126.784456	20.549287
62.957933	2118.520564	20.554304
62.715839	2116.541692	20.559322
62.752940	2126.647840	20.564339
62.870811	2133.383282	20.569357
63.377379	2144.593101	20.574375
63.152355	2154.427883	20.579392
63.617244	2152.170968	20.584410
63.299530	2160.574794	20.589427
63.090423	2147.553964	20.594445
63.401525	2148.928535	20.599463
63.293101	2141.658078	20.604480
63.250261	2142.791431	20.609498
63.344370	2173.112784	20.614515
63.592723	2169.176044	20.619533
63.764831	2166.614675	20.624551
63.818531	2168.746004	20.629568
63.954040	2171.413673	20.634586
63.771082	2180.474952	20.639603
63.908144	2172.556899	20.644621
64.093108	2174.636102	20.649639
64.232896	2189.050022	20.654656
64.512683	2192.143252	20.659674
64.249860	2199.556956	20.664691
64.616873	2185.940862	20.669709
64.252475	2199.433306	20.674727
64.408293	2202.949940	20.679744
64.674985	2195.469199	20.684762
64.774290	2200.866241	20.689779
64.356607	2190.759560	20.694797
64.377120	2191.507417	20.699815
64.664499	2196.944426	20.704832
64.782806	2205.374642	20.709850
64.730764	2216.788801	20.714867
65.036299	2213.060862	20.719885
64.797142	2208.622931	20.724903
65.115738	2220.878506	20.729920
65.027407	2213.601717	20.734938
65.275565	2212.199333	20.739955
65.341120	2203.232026	20.744973
65.312713	2224.445277	20.749991
65.187405	2236.404305	20.755008
65.448296	2235.612206	20.760026
65.407154	2242.539875	20.765043
65.724553	2232.826132	20.770061
65.701100	2236.863208	20.775079
65.698259	2238.365875	20.780096
65.887487	2231.279142	20.785114
65.837267	2251.233408	20.790131
66.338052	2243.671785	20.795149
66.228773	2255.634628	20.800167
66.461970	2258.504775	20.805184
66.663009	2254.089391	20.810202
66.179830	2256.336407	20.815219
66.526994	2254.211544	20.820237
66.334025	2256.144823	20.825255
66.769790	2250.805804	20.830272
67.063375	2248.326386	20.835290
66.435563	2249.999559	20.840307
66.930470	2253.983831	20.845325
67.130324	2251.724244	20.850343
66.677248	2247.414501	20.855360
66.756737	2254.399021	20.860378
66.682475	2255.960220	20.865395
66.848871	2248.157469	20.870413
66.970461	2246.819098	20.875431
67.001810	2248.767729	20.880448
66.864930	2244.111775	20.885466
67.102315	2260.410426	20.890483
67.390310	2261.204749	20.895501
67.372135	2263.022273	20.900519
67.332684	2271.483549	20.905536
67.802459	2273.155191	20.910554
67.903385	2274.884621	20.915571
67.655417	2274.809776	20.920589
67.884952	2267.053934	20.925607
67.689146	2269.741966	20.930624
68.032034	2277.455313	20.935642
67.746165	2278.585722	20.940659
67.802021	2278.116105	20.945677
68.165471	2275.272254	20.950695
67.899184	2284.046811	20.955712
67.767257	2287.652729	20.960730
67.987757	2298.822250	20.965747
68.039956	2288.354691	20.970765
68.323465	2298.977803	20.975783
68.014238	2300.651565	20.980800
68.303917	2306.201867	20.985818
68.026630	2316.243759	20.990835
68.554927	2327.412415	20.995853
68.459689	2329.885864	21.000871
68.460645	2332.984932	21.005888
68.692608	2326.147111	21.010906
68.643997	2342.882002	21.015923
68.882301	2346.445706	21.020941
69.147730	2353.047649	21.025959
68.966735	2358.599119	21.030976
69.574330	2347.337541	21.035994
69.275726	2347.639892	21.041011
69.457857	2351.120872	21.046029
69.393067	2345.064910	21.051047
69.398493	2353.973672	21.056064
69.418751	2346.256897	21.061082
69.479675	2355.103312	21.066099
69.316404	2355.346587	21.071117
70.190506	2372.804871	21.076135
69.487026	2366.763753	21.081152
69.861392	2369.668610	21.086170
69.828135	2365.741232	21.091187
70.062495	2364.372559	21.096205
70.193764	2361.208432	21.101223
70.137636	2370.960060	21.106240
70.293269	2368.656889	21.111258
69.978996	2371.224626	21.116275
70.387483	2371.725495	21.121293
70.830944	2382.863292	21.126311
70.343660	2385.603320	21.131328
70.474005	2380.867589	21.136346
70.781291	2383.700900	21.141363
71.009073	2378.176658	21.146381
70.648332	2382.408636	21.151399
70.713955	2383.354581	21.156416
71.070063	2385.801509	21.161434
71.203305	2379.761851	21.166451
70.834287	2383.231347	21.171469
71.006742	2388.112008	21.176487
70.952474	2406.754137	21.181504
71.239067	2406.942712	21.186522
71.329766	2403.052715	21.191539
71.332267	2414.392175	21.196557
71.371298	2400.764183	21.201575
71.162384	2409.782302	21.206592
71.453581	2423.847608	21.211610
71.710509	2430.570844	21.216627
71.722791	2431.111697	21.221645
72.273285	2431.467229	21.226663
71.720141	2435.104453	21.231680
71.938878	2432.497867	21.236698
72.148536	2427.954846	21.241715
72.091176	2428.626542	21.246733
71.978463	2429.922354	21.251751
71.936224	2439.255235	21.256768
71.951374	2440.471048	21.261786
72.403232	2451.493952	21.266803
72.216931	2458.034150	21.271821
72.503475	2450.843713	21.276839
72.515774	2459.259096	21.281856
72.550749	2454.383638	21.286874
72.779578	2459.381731	21.291891
72.860119	2474.313298	21.296909
73.034208	2471.868353	21.301927
73.298351	2485.114197	21.306944
72.923596	2478.033669	21.311962
73.165566	2475.988384	21.316979
73.308217	2475.287391	21.321997
73.672618	2474.409629	21.327015
73.585650	2480.643909	21.332032
73.542226	2478.239353	21.337050
73.796438	2477.789152	21.342067
73.645346	2476.323055	21.347085
73.655951	2470.384639	21.352103
73.478439	2477.087586	21.357120
73.671954	2469.564543	21.362138
73.904446	2475.360566	21.367155
73.853002	2473.604274	21.372173
74.290768	2480.330757	21.377191
74.008546	2481.413264	21.382208
73.848196	2485.639120	21.387226
73.786996	2495.700911	21.392243
73.701622	2501.953885	21.397261
74.142677	2490.986582	21.402279
74.423862	2508.411647	21.407296
74.269481	2526.564605	21.412314
74.216794	2522.589737	21.417331
74.520704	2535.608459	21.422349
74.588162	2525.406643	21.427367
74.494573	2527.141324	21.432384
74.402344	2542.614467	21.437402
74.982491	2539.682971	21.442419
74.988425	2546.294080	21.447437
75.434402	2538.526305	21.452455
75.197222	2542.934642	21.457472
75.493858	2533.523825	21.462490
75.222347	2540.115276	21.467507
75.410506	2546.085544	21.472525
75.698174	2542.641234	21.477543
75.438086	2552.036709	21.482560
75.705862	2554.390192	21.487578
75.908042	2558.398303	21.492595
76.029375	2569.984359	21.497613
76.141074	2563.430407	21.502631
76.167324	2572.159271	21.507648
76.439108	2561.155323	21.512666
76.097495	2554.896482	21.517683
76.066520	2562.220355	21.522701
75.825935	2559.329071	21.527719
76.162717	2560.046329	21.532736
76.274082	2562.711527	21.537754
76.434353	2563.112420	21.542771
76.299985	2583.130736	21.547789
76.658670	2579.804695	21.552807
76.470077	2578.735827	21.557824
76.871717	2580.560200	21.562842
76.790348	2578.158420	21.567859
76.572992	2585.451536	21.572877
76.951965	2580.452714	21.577895
77.194610	2599.727097	21.582912
77.454562	2596.356555	21.587930
77.463211	2598.390840	21.592947
77.566222	2608.360687	21.597965
77.483678	2611.087835	21.602983
77.445112	2598.109394	21.608000
77.440370	2604.267711	21.613018
77.483869	2600.517624	21.618035
77.274559	2594.067609	21.623053
77.718907	2598.334465	21.628071
77.686892	2598.118474	21.633088
77.509295	2606.904542	21.638106
77.980040	2618.871436	21.643123
78.019063	2621.936184	21.648141
78.143993	2620.559388	21.653159
78.496781	2625.184617	21.658176
78.345118	2618.441507	21.663194
78.743166	2617.839365	21.668211
78.633337	2625.756351	21.673229
78.713455	2615.246353	21.678247
78.760239	2618.606563	21.683264
78.447057	2614.476806	21.688282
78.668291	2604.538063	21.693299
78.841704	2611.151361	21.698317
78.487985	2611.355042	21.703335
78.987203	2624.737748	21.708352
78.934336	2632.664749	21.713370
79.528441	2637.331078	21.718387
79.242187	2645.392490	21.723405
79.249530	2647.688947	21.728423
79.453698	2650.936133	21.733440
79.142693	2643.091229	21.738458
79.505417	2640.247437	21.743475
79.570553	2659.489728	21.748493
79.684891	2656.211424	21.753511
79.596554	2667.315938	21.758528
79.864987	2665.588416	21.763546
80.144615	2659.853970	21.768563
79.811248	2665.735554	21.773581
79.701067	2673.286500	21.778599
79.844157	2673.213507	21.783616
80.130396	2682.902196	21.788634
80.432707	2687.806779	21.793651
80.280106	2701.320070	21.798669
80.704155	2697.033760	21.803687
80.763508	2691.930331	21.808704
80.469920	2681.096949	21.813722
80.727131	2691.553982	21.818739
80.795934	2710.944093	21.823757
80.802568	2707.177667	21.828775
80.897160	2716.246228	21.833792
81.125846	2715.137225	21.838810
81.243570	2716.633667	21.843827
80.747282	2724.930016	21.848845
81.001573	2713.439510	21.853863
81.066177	2721.348145	21.858880
81.340229	2737.243808	21.863898
81.698465	2732.055667	21.868915
81.477946	2734.119559	21.873933
81.207866	2736.977105	21.878951
81.255849	2746.917776	21.883968
81.556226	2767.025992	21.888986
81.591847	2756.374543	21.894003
82.101643	2759.946295	21.899021
82.308069	2749.492178	21.904039
82.480720	2746.734960	21.909056
82.063292	2759.336619	21.914074
82.600404	2764.927202	21.919091
82.661603	2774.730103	21.924109
82.711661	2784.585253	21.929127
82.938534	2767.654593	21.934144
83.146769	2783.724729	21.939162
83.166809	2778.583248	21.944179
83.136362	2774.374440	21.949197
83.007717	2771.607611	21.954215
83.092579	2771.922482	21.959232
83.138196	2773.771093	21.964250
83.025964	2766.182206	21.969267
82.845778	2781.205376	21.974285
83.115386	2778.205717	21.979303
83.290975	2768.078352	21.984320
83.009086	2775.949768	21.989338
83.032449	2780.194252	21.994355
83.332946	2802.205667	21.999373
83.598036	2793.920102	22.004391
83.778674	2794.642897	22.009408
83.382695	2806.455339	22.014426
83.683279	2804.779577	22.019443
83.888173	2816.630446	22.024461
83.782533	2818.944626	22.029479
84.143335	2821.671781	22.034496
83.938875	2837.358444	22.039514
84.435041	2841.696146	22.044531
84.486450	2847.353382	22.049549
84.378372	2847.701639	22.054567
84.799320	2838.305905	22.059584
84.581619	2846.056829	22.064602
85.149399	2838.209875	22.069619
84.816662	2838.110432	22.074637
85.026114	2854.742243	22.079655
85.246517	2854.818103	22.084672
85.681522	2864.126932	22.089690
85.745270	2854.727185	22.094707
85.727936	2872.174124	22.099725
85.268949	2865.488539	22.104743
85.538852	2861.049594	22.109760
85.665706	2861.392606	22.114778
85.813191	2859.377864	22.119795
85.566640	2854.925148	22.124813
85.733793	2858.680006	22.129831
86.184698	2850.513645	22.134848
85.764177	2857.744016	22.139866
86.062317	2870.154738	22.144883
86.015385	2881.814701	22.149901
86.105251	2887.727890	22.154919
86.537716	2883.736901	22.159936
86.342873	2886.383842	22.164954
86.614014	2888.023541	22.169971
86.392128	2891.100806	22.174989
86.448724	2900.705655	22.180007
86.749686	2900.207089	22.185024
86.861632	2907.281464	22.190042
86.819968	2908.831300	22.195059
86.699320	2908.449287	22.200077
86.674347	2909.964946	22.205095
87.016755	2928.756933	22.210112
87.381550	2939.759060	22.215130
87.380919	2934.488213	22.220147
87.190368	2940.735724	22.225165
87.626239	2947.465837	22.230183
87.775774	2956.532224	22.235200
87.652591	2971.694963	22.240218
87.966813	2960.927152	22.245235
88.237115	2961.897872	22.250253
88.078210	2969.623855	22.255271
88.581034	2955.323100	22.260288
88.261166	2955.767665	22.265306
88.282174	2952.753271	22.270323
88.322078	2954.271393	22.275341
88.292705	2968.008605	22.280359
88.365660	2951.950909	22.285376
88.690593	2969.571566	22.290394
88.726439	2977.497444	22.295411
88.650215	2980.615027	22.300429
88.435437	2986.361355	22.305447
88.802670	2980.733019	22.310464
88.786809	2980.271464	22.315482
89.375343	2983.742551	22.320499
89.474360	2979.267226	22.325517
89.443914	2984.031496	22.330535
89.884590	2990.782967	22.335552
89.437223	2991.405318	22.340570
89.666748	2997.403974	22.345587
89.879069	3005.317997	22.350605
89.755754	3006.845915	22.355623
89.886088	3004.297286	22.360640
89.706388	3003.372184	22.365658
89.880068	3002.846214	22.370675
90.043627	3007.384409	22.375693
89.918288	3001.631241	22.380711
90.089658	3015.557974	22.385728
90.298365	3030.485704	22.390746
90.476861	3025.032111	22.395763
90.402846	3027.363457	22.400781
90.218268	3032.132950	22.405799
90.493000	3036.435955	22.410816
90.524892	3046.925340	22.415834
90.657417	3053.248522	22.420851
91.266077	3051.325629	22.425869
90.777044	3057.673599	22.430887
91.083315	3062.388292	22.435904
91.122587	3069.663491	22.440922
91.236039	3071.593035	22.445939
91.375945	3076.835637	22.450957
91.578760	3080.465018	22.455975
91.732681	3074.567075	22.460992
91.659041	3082.560652	22.466010
91.848002	3093.590423	22.471027
91.762557	3095.907786	22.476045
91.896840	3096.363263	22.481063
92.053999	3098.099746	22.486080
92.015296	3106.551827	22.491098
92.158295	3100.908086	22.496115
92.049171	3108.897766	22.501133
92.309007	3114.992712	22.506151
92.608390	3110.829993	22.511168
92.680200	3116.733461	22.516186
92.606578	3116.568170	22.521203
92.689741	3120.288898	22.526221
92.713267	3136.394600	22.531239
92.916637	3146.184897	22.536256
93.193129	3141.631228	22.541274
93.094950	3139.058412	22.546291
93.483685	3137.050029	22.551309
92.987981	3145.396978	22.556327
93.405035	3163.495767	22.561344
93.309851	3154.505826	22.566362
93.575247	3162.310603	22.571379
93.905894	3168.735348	22.576397
93.897652	3164.791251	22.581415
94.087163	3164.890890	22.586432
93.752159	3165.659768	22.591450
94.245026	3171.945474	22.596467
94.345510	3180.360003	22.601485
94.190395	3190.755676	22.606503
94.652050	3186.141423	22.611520
94.616615	3191.263185	22.616538
94.299841	3180.155384	22.621555
94.760148	3182.298880	22.626573
94.472219	3206.066323	22.631591
94.813495	3210.690352	22.636608
95.070020	3213.152998	22.641626
94.660879	3214.043961	22.646643
95.117542	3211.292676	22.651661
94.819171	3217.462487	22.656679
95.395527	3226.515796	22.661696
95.346079	3233.795492	22.666714
95.397904	3239.481193	22.671731
95.690073	3235.647828	22.676749
95.575174	3247.700583	22.681767
95.605152	3241.070813	22.686784
95.816251	3244.601085	22.691802
95.646637	3252.780212	22.696819
96.004780	3258.948181	22.701837
95.955961	3255.351298	22.706855
95.456824	3247.036914	22.711872
96.257665	3270.595988	22.716890
96.518106	3279.982883	22.721907
96.479437	3271.261782	22.726925
96.593769	3280.845163	22.731943
96.767298	3289.825896	22.736960
97.001429	3294.753954	22.741978
97.123004	3300.965312	22.746995
97.150736	3307.806849	22.752013
97.191792	3320.068783	22.757031
97.378534	3308.181323	22.762048
97.678268	3302.478245	22.767066
97.562927	3308.572066	22.772083
97.733164	3308.318067	22.777101
97.497638	3303.162820	22.782119
97.665954	3305.894957	22.787136
97.609163	3317.812404	22.792154
97.587087	3318.450198	22.797171
97.893534	3338.015222	22.802189
98.076528	3336.190553	22.807207
98.224104	3334.014773	22.812224
98.324460	3338.414609	22.817242
98.231991	3355.630753	22.822259
98.651558	3353.974176	22.827277
98.652790	3357.591007	22.832295
98.597853	3353.187054	22.837312
98.745064	3352.810411	22.842330
98.957505	3360.932887	22.847347
99.433042	3370.052565	22.852365
99.393917	3375.711526	22.857383
99.183495	3375.498226	22.862400
99.572047	3377.514112	22.867418
99.263626	3372.771113	22.872435
99.741253	3373.649406	22.877453
99.453733	3373.280902	22.882471
99.721028	3380.299561	22.887488
99.495384	3372.690311	22.892506
99.672187	3391.161535	22.897523
100.284966	3395.594730	22.902541
99.867633	3400.022030	22.907559
99.836262	3398.082594	22.912576
100.074943	3403.751697	22.917594
99.961555	3429.666772	22.922611
100.291763	3425.448652	22.927629
100.509496	3415.721485	22.932647
100.518253	3425.239419	22.937664
100.692041	3445.039971	22.942682
100.633453	3456.916759	22.947699
100.950173	3455.945423	22.952717
101.164286	3452.177899	22.957735
101.034006	3450.519082	22.962752
101.347541	3455.706186	22.967770
101.161203	3470.601483	22.972787
101.738000	3470.687793	22.977805
101.918474	3464.719281	22.982823
102.021016	3467.531186	22.987840
101.899124	3471.328301	22.992858
101.916066	3475.166791	22.997875
102.184931	3465.153832	23.002893
102.040560	3458.753301	23.007911
102.065704	3470.986267	23.012928
102.505157	3472.760623	23.017946
102.348588	3488.831729	23.022963
102.660119	3488.195772	23.027981
102.399081	3491.080424	23.032999
102.412260	3488.120825	23.038016
102.782471	3486.853882	23.043034
102.640130	3495.205599	23.048051
102.589836	3503.318801	23.053069
102.754081	3516.341176	23.058087
102.714154	3509.065748	23.063104
103.295834	3516.069925	23.068122
102.888390	3540.683484	23.073139
103.256788	3539.410510	23.078157
103.620913	3538.561152	23.083175
103.225454	3540.485258	23.088192
103.551163	3554.681764	23.093210
103.876425	3569.560116	23.098227
104.086637	3558.208546	23.103245
104.174604	3567.938245	23.108263
104.081102	3557.925192	23.113280
104.670968	3577.641765	23.118298
104.101805	3594.314179	23.123315
104.255175	3589.325177	23.128333
104.820174	3586.515832	23.133351
104.904332	3590.608948	23.138368
105.209339	3591.059785	23.143386
104.885552	3589.664840	23.148403
105.028004	3599.029355	23.153421
105.198606	3606.183192	23.158439
105.402651	3620.209431	23.163456
105.510203	3611.720920	23.168474
105.386058	3617.027143	23.173491
105.919286	3619.616936	23.178509
105.883935	3615.373980	23.183527
105.661521	3623.523671	23.188544
105.838011	3633.226910	23.193562
106.043622	3635.785969	23.198579
106.445300	3629.962658	23.203597
106.447259	3632.127518	23.208615
106.504383	3637.910360	23.213632
106.538528	3630.004637	23.218650
106.356152	3643.166630	23.223667
106.661114	3660.172450	23.228685
106.759507	3667.012521	23.233703
106.603279	3657.593163	23.238720
106.906068	3656.071641	23.243738
106.834920	3663.774701	23.248755
107.065867	3670.177370	23.253773
107.047582	3688.029256	23.258791
107.308031	3688.023096	23.263808
107.575882	3681.766222	23.268826
107.108306	3687.018954	23.273843
107.613181	3703.993495	23.278861
107.866461	3706.781822	23.283879
107.630635	3704.123175	23.288896
107.994084	3712.553567	23.293914
107.836653	3726.917436	23.298931
107.944172	3734.106457	23.303949
108.271424	3731.337495	23.308967
108.365310	3742.915980	23.313984
108.935835	3750.673209	23.319002
108.800815	3759.124903	23.324019
108.627382	3756.961489	23.329037
109.295463	3766.726663	23.334055
108.809418	3763.797886	23.339072
109.486298	3757.249646	23.344090
109.424850	3753.247473	23.349107
109.370523	3757.665333	23.354125
109.563771	3757.590792	23.359143
109.359017	3762.695054	23.364160
109.695777	3762.295019	23.369178
109.924924	3781.926292	23.374195
109.944976	3782.112456	23.379213
109.788664	3786.110723	23.384231
109.926993	3772.302009	23.389248
110.019067	3779.382996	23.394266
110.345697	3783.637018	23.399283
110.134537	3803.905442	23.404301
110.345375	3802.003769	23.409319
110.344518	3805.737802	23.414336
110.415778	3808.693541	23.419354
110.550868	3825.950232	23.424371
110.782633	3830.941935	23.429389
110.974989	3830.302544	23.434407
110.467038	3833.762516	23.439424
111.314066	3842.899986	23.444442
111.446844	3853.238309	23.449459
111.413226	3850.229167	23.454477
111.624881	3843.062539	23.459495
111.542409	3854.596129	23.464512
111.728933	3856.858355	23.469530
112.098749	3871.382776	23.474547
112.161436	3864.548802	23.479565
112.211708	3869.928777	23.484583
112.512700	3865.604660	23.489600
112.697755	3869.950324	23.494618
112.720621	3882.253365	23.499635
112.843365	3891.280230	23.504653
112.946605	3888.218077	23.509671
113.110481	3892.374524	23.514688
112.903195	3893.770478	23.519706
113.316931	3890.801716	23.524723
113.368088	3883.508711	23.529741
113.395061	3876.692953	23.534759
113.118860	3896.192046	23.539776
113.371783	3905.908708	23.544794
113.435174	3916.052774	23.549811
113.433674	3911.665564	23.554829
113.836920	3921.554380	23.559847
113.727990	3942.173082	23.564864
113.835581	3933.403497	23.569882
114.207609	3940.519596	23.574899
114.266409	3950.225662	23.579917
114.596425	3966.110485	23.584935
114.397906	3982.466362	23.589952
114.719117	3972.773187	23.594970
114.976375	3963.778130	23.599987
115.023542	3961.687448	23.605005
115.048770	3969.694334	23.610023
115.015396	3996.127957	23.615040
115.329241	3997.107696	23.620058
115.057990	3998.362171	23.625075
115.514694	3996.911200	23.630093
115.451630	4004.259622	23.635111
115.150658	4023.264021	23.640128
115.543725	4016.744373	23.645146
115.656908	4032.495935	23.650163
115.599322	4051.768404	23.655181
116.168255	4050.138869	23.660199
116.153419	4049.759192	23.665216
116.430245	4045.246279	23.670234
116.184337	4049.902547	23.675251
116.242977	4065.489081	23.680269
116.858415	4071.768527	23.685287
116.758933	4072.206995	23.690304
116.575484	4078.943027	23.695322
117.333737	4086.730962	23.700339
116.828300	4095.606988	23.705357
117.265120	4098.868491	23.710375
117.237167	4103.556910	23.715392
117.616209	4096.231389	23.720410
117.530467	4100.831013	23.725427
117.676981	4118.767978	23.730445
117.884465	4125.089262	23.735463
117.514602	4126.861066	23.740480
117.645321	4133.841444	23.745498
117.928015	4144.109100	23.750515
118.028771	4153.502529	23.755533
118.076179	4152.213518	23.760551
118.459889	4161.426896	23.765568
118.493324	4166.490797	23.770586
119.221616	4168.150531	23.775603
118.924047	4175.633612	23.780621
119.000254	4174.475814	23.785639
119.102083	4191.561305	23.790656
119.624642	4195.254449	23.795674
119.653977	4192.696226	23.800691
119.673112	4191.724128	23.805709
119.884828	4193.433231	23.810727
119.995099	4193.848310	23.815744
119.922260	4191.454447	23.820762
120.023505	4207.571021	23.825779
119.727584	4223.513099	23.830797
120.352311	4213.803810	23.835815
120.375301	4223.294683	23.840832
120.621091	4221.643161	23.845850
121.103047	4235.566366	23.850867
120.752986	4240.696683	23.855885
120.788433	4235.751230	23.860903
121.020895	4239.587682	23.865920
121.014367	4235.848252	23.870938
121.332624	4234.223253	23.875955
121.231135	4250.643081	23.880973
121.671586	4261.201732	23.885991
121.105336	4268.313450	23.891008
121.151075	4263.309562	23.896026
121.601379	4280.671968	23.901043
121.881353	4280.356575	23.906061
122.020948	4283.061796	23.911079
121.891654	4300.568685	23.916096
121.734368	4299.441147	23.921114
122.156734	4304.693514	23.926131
122.314070	4326.438823	23.931149
122.935671	4333.474944	23.936167
122.859750	4348.574613	23.941184
122.621786	4349.085287	23.946202
123.021948	4338.454708	23.951219
122.833005	4351.463575	23.956237
123.234579	4365.592017	23.961255
123.269541	4366.748041	23.966272
123.472743	4360.905090	23.971290
123.538811	4377.462917	23.976307
124.074973	4395.241260	23.981325
124.177985	4389.439249	23.986343
124.202075	4389.034527	23.991360
124.055778	4397.141074	23.996378
124.259239	4393.775896	24.001395
124.488745	4409.307548	24.006413
124.529931	4412.555336	24.011431
124.793154	4426.292003	24.016448
125.074197	4421.068132	24.021466
125.259675	4423.523138	24.026483
125.323084	4417.818859	24.031501
125.143780	4418.171990	24.036519
125.165512	4417.139501	24.041536
125.009763	4411.649478	24.046554
125.422052	4434.077804	24.051571
125.127270	4450.291358	24.056589
125.233471	4443.030539	24.061607
125.470127	4454.527139	24.066624
125.294686	4468.323093	24.071642
125.988009	4477.327145	24.076659
126.244481	4494.735907	24.081677
126.341908	4501.816337	24.086695
126.420342	4496.851453	24.091712
126.579017	4503.524572	24.096730
126.785084	4491.746945	24.101747
126.526376	4529.460032	24.106765
127.024788	4522.260838	24.111783
127.480142	4520.787943	24.116800
127.208916	4526.660389	24.121818
127.438962	4523.373091	24.126835
127.396498	4548.527408	24.131853
127.529625	4539.589393	24.136871
127.624026	4540.107973	24.141888
127.727950	4551.729594	24.146906
127.996055	4565.762312	24.151923
128.110730	4571.277604	24.156941
128.126352	4570.489113	24.161959
128.441507	4574.666208	24.166976
128.345576	4585.735209	24.171994
128.679228	4593.757181	24.177011
128.754707	4597.056447	24.182029
128.685562	4602.234392	24.187047
128.970008	4609.673815	24.192064
129.097808	4621.866222	24.197082
129.248097	4614.740471	24.202099
129.370032	4619.635965	24.207117
129.669094	4632.054069	24.212135
129.989073	4632.575190	24.217152
129.793728	4642.337225	24.222170
130.211815	4637.369594	24.227187
130.024289	4647.101998	24.232205
129.733637	4649.697915	24.237223
129.980376	4665.413321	24.242240
130.312837	4663.423062	24.247258
130.684188	4663.405842	24.252275
130.720077	4681.527990	24.257293
130.899119	4684.252344	24.262311
131.070475	4693.152045	24.267328
130.656842	4694.533038	24.272346
131.297358	4701.853584	24.277363
131.549888	4714.973468	24.282381
131.201127	4716.824090	24.287399
131.477669	4716.985863	24.292416
131.552772	4734.723138	24.297434
131.746271	4746.807485	24.302451
132.059569	4750.647164	24.307469
131.973230	4753.220556	24.312487
132.434211	4765.319827	24.317504
132.187223	4764.398861	24.322522
132.425782	4762.912565	24.327539
132.774425	4781.165736	24.332557
132.667866	4788.896916	24.337575
132.961878	4788.762395	24.342592
133.053109	4796.481531	24.347610
133.280120	4793.718645	24.352627
133.295940	4796.386518	24.357645
133.427996	4810.551218	24.362663
133.908013	4812.382487	24.367680
133.600354	4814.554960	24.372698
133.969505	4821.946477	24.377715
134.065989	4821.726110	24.382733
134.182764	4812.998854	24.387751
134.526105	4837.158793	24.392768
134.331865	4839.357690	24.397786
134.749281	4838.742981	24.402803
134.574970	4840.427397	24.407821
134.570582	4836.040417	24.412839
134.600382	4849.877106	24.417856
135.007974	4866.132506	24.422874
135.028677	4871.864630	24.427891
135.001242	4882.140256	24.432909
134.830290	4893.142283	24.437927
135.345551	4892.060857	24.442944
135.312924	4911.011514	24.447962
135.694598	4916.882807	24.452979
135.558287	4925.313147	24.457997
135.806903	4937.505778	24.463015
136.014529	4951.068473	24.468032
136.554821	4958.306972	24.473050
135.982690	4964.261421	24.478067
136.799887	4974.275355	24.483085
136.929317	4977.020152	24.488103
137.311101	4979.899025	24.493120
136.950747	4996.574726	24.498138
137.465647	5003.283762	24.503155
137.661880	5004.995369	24.508173
137.467338	5003.513774	24.513191
137.914173	5009.507464	24.518208
137.761155	5015.424678	24.523226
137.963962	5012.542445	24.528243
137.960561	5024.998734	24.533261
138.179289	5025.983963	24.538279
138.406007	5033.012780	24.543296
138.571956	5048.466551	24.548314
138.349040	5052.412398	24.553331
138.750307	5061.235225	24.558349
138.818521	5067.954289	24.563367
138.899394	5069.668193	24.568384
138.841326	5077.060457	24.573402
139.232882	5077.081108	24.578419
139.250519	5100.064512	24.583437
139.144322	5102.574776	24.588455
139.543502	5109.159934	24.593472
139.953680	5130.528838	24.598490
140.130815	5137.511801	24.603507
139.932674	5132.318607	24.608525
140.103327	5147.134094	24.613543
140.518554	5151.993253	24.618560
140.554122	5169.478304	24.623578
140.508887	5166.814833	24.628595
140.940928	5170.762263	24.633613
141.213572	5176.183545	24.638631
141.745463	5187.422864	24.643648
141.711008	5185.010230	24.648666
141.570074	5182.150257	24.653683
141.498655	5187.376073	24.658701
141.585631	5188.861756	24.663719
142.044251	5201.668768	24.668736
142.000552	5206.410443	24.673754
142.213918	5206.152821	24.678771
142.634029	5214.297257	24.683789
142.188147	5216.188396	24.688807
142.439571	5221.499379	24.693824
142.484703	5237.606717	24.698842
142.632245	5229.152223	24.703859
143.006439	5241.461119	24.708877
142.721374	5249.949637	24.713895
142.757367	5255.038693	24.718912
143.058685	5257.857616	24.723930
143.545924	5272.664643	24.728947
143.841424	5284.771246	24.733965
143.517902	5291.693813	24.738983
143.632319	5289.832346	24.744000
144.054033	5302.260102	24.749018
143.803755	5307.674962	24.754035
144.131907	5313.280143	24.759053
144.234013	5324.921481	24.764071
144.796503	5329.082100	24.769088
144.687972	5337.751339	24.774106
144.791929	5334.786687	24.779123
145.065331	5356.022609	24.784141
144.877971	5366.036309	24.789159
145.274397	5364.253762	24.794176
145.667071	5382.380687	24.799194
145.756965	5387.227746	24.804211
145.776175	5388.891363	24.809229
145.682020	5400.026869	24.814247
146.315538	5406.266072	24.819264
146.194202	5423.864335	24.824282
146.279822	5419.725114	24.829299
146.530854	5421.769093	24.834317
146.291520	5436.506997	24.839335
146.901340	5441.818716	24.844352
147.001789	5439.242864	24.849370
146.951425	5455.387451	24.854387
147.396539	5458.666844	24.859405
146.912160	5465.466314	24.864423
147.606375	5468.570948	24.869440
147.607738	5475.991942	24.874458
147.905073	5476.314612	24.879475
148.041633	5483.203052	24.884493
148.121284	5508.538430	24.889511
148.566237	5511.076044	24.894528
148.142989	5507.445831	24.899546
148.446980	5528.244699	24.904563
149.178169	5538.244012	24.909581
148.895207	5541.012465	24.914599
149.325962	5543.293462	24.919616
149.201709	5552.609225	24.924634
149.361821	5559.654993	24.929651
149.819646	5570.884057	24.934669
149.727776	5564.828104	24.939687
150.237993	5565.363644	24.944704
149.902177	5574.614706	24.949722
149.934110	5593.600150	24.954739
150.213674	5591.621237	24.959757
150.070711	5588.745735	24.964775
150.366232	5604.893086	24.969792
150.521474	5610.560171	24.974810
150.645414	5617.889417	24.979827
150.948301	5627.431871	24.984845
151.059760	5642.187587	24.989863
151.239305	5642.446640	24.994880
151.075990	5661.027121	24.999898
151.438313	5675.513124	25.004915
151.719743	5675.582599	25.009933
151.371954	5688.885621	25.014951
151.910479	5695.682757	25.019968
151.883158	5706.154544	25.024986
152.029338	5719.686400	25.030003
152.583223	5732.977619	25.035021
152.451122	5733.178170	25.040039
153.051848	5743.030731	25.045056
153.096184	5751.540479	25.050074
153.129196	5763.237115	25.055091
153.214500	5753.961918	25.060109
153.208943	5761.324135	25.065127
153.628153	5770.677979	25.070144
153.532128	5780.200934	25.075162
153.573115	5785.784959	25.080179
153.931341	5782.600468	25.085197
153.955069	5799.178846	25.090215
154.280983	5800.529289	25.095232
154.628382	5806.384144	25.100250
154.583824	5822.032542	25.105267
155.037324	5830.389837	25.110285
154.855236	5833.473985	25.115303
154.823718	5823.042758	25.120320
155.404990	5853.429684	25.125338
155.721955	5853.436772	25.130355
155.870039	5856.535489	25.135373
155.875582	5850.678836	25.140391
155.811693	5852.810082	25.145408
155.737218	5868.201199	25.150426
155.917214	5871.844187	25.155443
156.267108	5875.709941	25.160461
156.480363	5903.079960	25.165479
156.619649	5898.329290	25.170496
156.505826	5905.380227	25.175514
156.339647	5933.100153	25.180531
157.029482	5928.140112	25.185549
157.094763	5942.663393	25.190567
157.519287	5949.961465	25.195584
157.675783	5956.341883	25.200602
157.543527	5967.111207	25.205619
158.088078	5986.913264	25.210637
158.327496	5990.616416	25.215655
158.108381	5986.916244	25.220672
158.607255	5986.872737	25.225690
158.580501	6000.700217	25.230707
159.182998	6012.610842	25.235725
159.258913	6013.353335	25.240743
159.042684	5996.391234	25.245760
159.134786	6010.951406	25.250778
159.147343	6021.003592	25.255795
159.136258	6033.218702	25.260813
159.179876	6044.235155	25.265831
159.665520	6055.261285	25.270848
159.575338	6069.344980	25.275866
159.837692	6093.475076	25.280883
160.244105	6092.312779	25.285901
160.373152	6109.755674	25.290919
160.509826	6117.291471	25.295936
160.788611	6118.399937	25.300954
161.240919	6130.454126	25.305971
161.181958	6138.336257	25.310989
161.200413	6146.645053	25.316007
161.349328	6157.714528	25.321024
161.865792	6158.009196	25.326042
161.760713	6165.743882	25.331059
161.803930	6172.217885	25.336077
161.920816	6179.340113	25.341095
162.318367	6185.859626	25.346112
162.684352	6186.010561	25.351130
162.646476	6195.777164	25.356147
162.716256	6191.681289	25.361165
162.679633	6201.936999	25.366183
163.012447	6213.040832	25.371200
163.314959	6208.191906	25.376218
163.231377	6218.480235	25.381235
163.586339	6236.617075	25.386253
163.696687	6246.767708	25.391271
164.032113	6242.387133	25.396288
164.423846	6245.580331	25.401306
163.977281	6257.718601	25.406323
164.281925	6263.577145	25.411341
164.458027	6279.516514	25.416359
164.679707	6277.439266	25.421376
164.696071	6280.946975	25.426394
164.604888	6297.029250	25.431411
164.982727	6292.727252	25.436429
164.884521	6308.097201	25.441447
164.997303	6317.871834	25.446464
165.335319	6322.216221	25.451482
165.511479	6341.463957	25.456499
165.867485	6343.621025	25.461517
166.014413	6355.464346	25.466535
166.226869	6375.473535	25.471552
166.491538	6376.388507	25.476570
166.586582	6384.855880	25.481587
166.852941	6401.639867	25.486605
167.061135	6410.499911	25.491623
167.198562	6401.569784	25.496640
167.235453	6403.375938	25.501658
167.181468	6421.191896	25.506675
167.529637	6424.486654	25.511693
167.895541	6436.794500	25.516711
168.015505	6447.180499	25.521728
168.458430	6446.811136	25.526746
167.909510	6455.979222	25.531763
168.591942	6471.899414	25.536781
168.768079	6475.157996	25.541799
168.574793	6483.077103	25.546816
168.665219	6495.437615	25.551834
168.790214	6519.927573	25.556851
169.096294	6523.143709	25.561869
169.284971	6534.901685	25.566887
169.400770	6545.705095	25.571904
170.066971	6564.156535	25.576922
169.913883	6562.251614	25.581939
170.005736	6553.581101	25.586957
170.463261	6577.914866	25.591975
170.339522	6586.602861	25.596992
170.945012	6590.892781	25.602010
170.852380	6603.878689	25.607027
170.923997	6611.301764	25.612045
171.320647	6617.521673	25.617063
170.805791	6624.203224	25.622080
171.247523	6636.284659	25.627098
171.538408	6651.079372	25.632115
171.705015	6665.704156	25.637133
171.978166	6664.426957	25.642151
172.178568	6682.894667	25.647168
172.597886	6685.490132	25.652186
172.613980	6701.088738	25.657203
172.856925	6702.269150	25.662221
173.098380	6708.567070	25.667239
173.077046	6729.730801	25.672256
173.322845	6723.918309	25.677274
173.115280	6736.433001	25.682292
173.724218	6749.672142	25.687309
173.943609	6744.495155	25.692327
173.940536	6753.303227	25.697344
174.237800	6760.694170	25.702362
174.375027	6776.984160	25.707380
174.601697	6770.723217	25.712397
174.683821	6775.527665	25.717415
174.700547	6792.215371	25.722432
175.180176	6801.238278	25.727450
175.294324	6799.739743	25.732468
175.353877	6798.997941	25.737485
175.638694	6815.249059	25.742503
175.281849	6825.403753	25.747520
175.788511	6820.355369	25.752538
175.712386	6839.889388	25.757556
175.774974	6849.760561	25.762573
176.364625	6860.953984	25.767591
176.381136	6878.715145	25.772608
176.596344	6892.177073	25.777626
176.675652	6894.488047	25.782644
176.657467	6903.791034	25.787661
177.095054	6906.011155	25.792679
176.911711	6931.026657	25.797696
177.469855	6929.104982	25.802714
177.548341	6948.245537	25.807732
177.920318	6966.626672	25.812749
177.885761	6968.466172	25.817767
177.885883	6992.272332	25.822784
178.248621	6989.566780	25.827802
178.734692	7007.964809	25.832820
178.750375	7028.024477	25.837837
179.295467	7025.268254	25.842855
179.234814	7032.889009	25.847872
179.649690	7045.467401	25.852890
179.790834	7048.157008	25.857908
179.707199	7051.052303	25.862925
179.829812	7063.641768	25.867943
179.959414	7071.662075	25.872960
179.841760	7079.503293	25.877978
180.201140	7101.059248	25.882996
180.660922	7104.674437	25.888013
180.959543	7118.997933	25.893031
181.194734	7123.516467	25.898048
181.124536	7134.399872	25.903066
181.187252	7134.822471	25.908084
181.380719	7157.342094	25.913101
182.005108	7151.710086	25.918119
181.997319	7167.811626	25.923136
182.124648	7169.259580	25.928154
181.919889	7181.063821	25.933172
182.430176	7198.530106	25.938189
182.781918	7203.503943	25.943207
182.403626	7215.461670	25.948224
183.044196	7227.521817	25.953242
183.195662	7238.231652	25.958260
183.295558	7240.864610	25.963277
183.501241	7250.934567	25.968295
183.674030	7264.125601	25.973312
183.949949	7271.248596	25.978330
184.132706	7291.882200	25.983348
184.317199	7295.142776	25.988365
184.418125	7300.635791	25.993383
184.151425	7320.607423	25.998400
184.375737	7333.203239	26.003418
184.884482	7343.074235	26.008436
184.983554	7353.558728	26.013453
185.549918	7358.985159	26.018471
185.692343	7379.224243	26.023488
185.660202	7382.004186	26.028506
185.890777	7391.060088	26.033524
185.894845	7398.206778	26.038541
186.272722	7405.891580	26.043559
186.540253	7423.809674	26.048576
186.485248	7437.882591	26.053594
186.544118	7446.214056	26.058612
186.771433	7459.226210	26.063629
187.456561	7455.134678	26.068647
187.519611	7468.368306	26.073664
187.521057	7476.052126	26.078682
187.940803	7485.772978	26.083700
187.764468	7489.481584	26.088717
188.330171	7504.372840	26.093735
188.080919	7506.549101	26.098752
188.404773	7503.795898	26.103770
188.623595	7529.948868	26.108788
188.728296	7534.314311	26.113805
188.525059	7538.352313	26.118823
188.776253	7548.314279	26.123840
189.396724	7576.232299	26.128858
189.692041	7581.578135	26.133876
190.002347	7591.811839	26.138893
190.444642	7588.528633	26.143911
190.318360	7610.833713	26.148928
190.281749	7610.359506	26.153946
190.535416	7616.662139	26.158964
190.939836	7632.879458	26.163981
191.444709	7636.200401	26.168999
190.930532	7642.910622	26.174016
191.294478	7664.147663	26.179034
191.678721	7666.180500	26.184052
191.921322	7683.496603	26.189069
192.013140	7687.535770	26.194087
191.859003	7699.884892	26.199104
192.346806	7709.330010	26.204122
192.556814	7719.753134	26.209140
192.318109	7734.404379	26.214157
192.815975	7747.039706	26.219175
192.842080	7761.873638	26.224192
192.970285	7777.626072	26.229210
193.101773	7777.829547	26.234228
192.937456	7794.496010	26.239245
193.593840	7808.366208	26.244263
193.841050	7823.743292	26.249280
194.107851	7835.871865	26.254298
194.891257	7851.947922	26.259316
194.994310	7875.657013	26.264333
194.940392	7857.821674	26.269351
194.887188	7868.930157	26.274368
195.027903	7883.193746	26.279386
195.624953	7888.909135	26.284404
195.679302	7903.937651	26.289421
195.947603	7914.140230	26.294439
196.066205	7918.730896	26.299456
196.309954	7937.612964	26.304474
196.452172	7949.300197	26.309492
196.508729	7960.555708	26.314509
197.268331	7961.803648	26.319527
197.159986	7965.978417	26.324544
197.118097	7985.685081	26.329562
197.809744	7989.377778	26.334580
198.024205	7991.762430	26.339597
198.220529	7993.420637	26.344615
198.150047	8006.997592	26.349632
198.427790	8018.430013	26.354650
198.483905	8017.736058	26.359668
198.445481	8029.442169	26.364685
198.808226	8039.206972	26.369703
198.934841	8053.229805	26.374720
198.832741	8065.233210	26.379738
199.365448	8072.818266	26.384756
199.316749	8091.597923	26.389773
199.783965	8096.910666	26.394791
200.022515	8104.810171	26.399808
199.958784	8118.790260	26.404826
200.247386	8125.835829	26.409844
200.568369	8139.348398	26.414861
200.708981	8149.549011	26.419879
200.756419	8160.648218	26.424896
201.075699	8168.370933	26.429914
201.150594	8176.106680	26.434932
200.987050	8192.495553	26.439949
201.178966	8206.823984	26.444967
201.486101	8224.079971	26.449984
201.747482	8235.732931	26.455002
202.159016	8244.615677	26.460020
202.198273	8261.168582	26.465037
202.173326	8276.721278	26.470055
202.525884	8288.479959	26.475072
202.671906	8309.467739	26.480090
202.990064	8313.237957	26.485108
203.309169	8333.725080	26.490125
203.654455	8355.540439	26.495143
203.696627	8363.483448	26.500160
203.919422	8384.295115	26.505178
204.308705	8379.722488	26.510196
204.534119	8399.788675	26.515213
204.996878	8408.480360	26.520231
205.094587	8421.286182	26.525248
205.372957	8428.276641	26.530266
205.808421	8428.460919	26.535284
205.971552	8448.817903	26.540301
206.270903	8461.551121	26.545319
206.070900	8454.807107	26.550336
206.201561	8466.521734	26.555354
206.796219	8480.301082	26.560372
206.417855	8488.032193	26.565389
206.852053	8498.666896	26.570407
207.146429	8503.811090	26.575424
207.614106	8513.373433	26.580442
207.489882	8521.487807	26.585460
207.724207	8542.351517	26.590477
208.365192	8539.422196	26.595495
208.400012	8551.590739	26.600512
208.071992	8563.655116	26.605530
208.601612	8563.562599	26.610548
208.606022	8593.555065	26.615565
208.668895	8591.758173	26.620583
209.089221	8613.890429	26.625600
209.338867	8627.004095	26.630618
209.684751	8636.522439	26.635636
209.846629	8650.622287	26.640653
210.020972	8663.110023	26.645671
210.062724	8675.747983	26.650688
210.073065	8685.322074	26.655706
210.407623	8699.742200	26.660724
210.260996	8711.159444	26.665741
210.981627	8732.278691	26.670759
210.895215	8740.273577	26.675776
210.728541	8765.901445	26.680794
211.448437	8776.513652	26.685812
211.727719	8798.813456	26.690829
211.800043	8806.350964	26.695847
212.505426	8826.746547	26.700864
212.463944	8835.365881	26.705882
212.931794	8840.331446	26.710900
213.113651	8858.760039	26.715917
213.110982	8858.419400	26.720935
213.584670	8881.872810	26.725952
213.597597	8892.267483	26.730970
213.706257	8889.168923	26.735988
213.781947	8905.378871	26.741005
213.933274	8914.492137	26.746023
214.444612	8920.836940	26.751040
214.345151	8925.619879	26.756058
214.591950	8941.660978	26.761076
214.614186	8955.255674	26.766093
215.427409	8971.340669	26.771111
215.575296	8986.267006	26.776128
215.454993	9001.715272	26.781146
216.055297	9004.049083	26.786164
215.754983	9024.207777	26.791181
215.844621	9026.855227	26.796199
216.235856	9039.176633	26.801216
216.307272	9054.310755	26.806234
217.155380	9068.237116	26.811252
217.412620	9078.378926	26.816269
217.276959	9096.945900	26.821287
217.335563	9106.045371	26.826304
217.509005	9129.334593	26.831322
217.766407	9127.813430	26.836340
218.225462	9147.187112	26.841357
218.089692	9160.838284	26.846375
218.444892	9175.716510	26.851392
218.495833	9184.312054	26.856410
218.870812	9206.695233	26.861428
219.263955	9225.056360	26.866445
219.447305	9236.873725	26.871463
219.931798	9248.378709	26.876480
220.056526	9273.478559	26.881498
220.427690	9274.190719	26.886516
220.823619	9298.963961	26.891533
220.444068	9307.942732	26.896551
220.323720	9313.208953	26.901568
220.590703	9330.611182	26.906586
221.371814	9350.218782	26.911604
221.404073	9359.600347	26.916621
221.242917	9368.825935	26.921639
221.890653	9387.144182	26.926656
222.066549	9410.881711	26.931674
222.406768	9423.650234	26.936692
222.615565	9435.280614	26.941709
222.950736	9453.654206	26.946727
223.529867	9467.790344	26.951744
223.234762	9475.581438	26.956762
223.917644	9480.952361	26.961780
223.817730	9494.762341	26.966797
223.844512	9504.189041	26.971815
224.213705	9521.051318	26.976832
224.525261	9538.314152	26.981850
224.686982	9546.766215	26.986868
225.080983	9555.945973	26.991885
224.883592	9577.096334	26.996903
225.349318	9577.601094	27.001920
225.603402	9596.003317	27.006938
225.783837	9613.450943	27.011956
226.302093	9625.490781	27.016973
226.277678	9642.755825	27.021991
226.569186	9638.081389	27.027008
226.977930	9657.573992	27.032026
227.204961	9665.479127	27.037044
227.510930	9671.891092	27.042061
226.995391	9689.899322	27.047079
227.416003	9707.479909	27.052096
227.592819	9715.910741	27.057114
227.980169	9729.635090	27.062132
228.682410	9751.304609	27.067149
228.345923	9762.689090	27.072167
228.848359	9769.158719	27.077184
229.056548	9779.668538	27.082202
229.223370	9784.558379	27.087220
229.445239	9796.587926	27.092237
229.896969	9807.994197	27.097255
230.216641	9821.451366	27.102272
230.456891	9830.308032	27.107290
230.525325	9826.388381	27.112308
230.766725	9846.210508	27.117325
230.465910	9854.488892	27.122343
231.015702	9865.096802	27.127360
230.951547	9881.187424	27.132378
231.488447	9893.833894	27.137396
231.953670	9907.145186	27.142413
231.879820	9913.531486	27.147431
232.265802	9924.446100	27.152448
232.313700	9939.991931	27.157466
232.698323	9958.762425	27.162484
232.411449	9971.455903	27.167501
232.627784	10001.622671	27.172519
232.965743	10007.609804	27.177536
232.912577	10030.604122	27.182554
233.183298	10052.761530	27.187572
233.934385	10069.412923	27.192589
233.988572	10096.128909	27.197607
234.134992	10107.602136	27.202624
234.423539	10123.634557	27.207642
234.566173	10151.025088	27.212660
234.828034	10161.599337	27.217677
235.422959	10183.586129	27.222695
235.737364	10195.828774	27.227712
236.100853	10213.879777	27.232730
236.014196	10222.557347	27.237748
236.549765	10244.528250	27.242765
236.339630	10248.997330	27.247783
237.250555	10261.557042	27.252800
237.179908	10280.787548	27.257818
237.274530	10293.813007	27.262836
237.712348	10304.413450	27.267853
237.544470	10326.201001	27.272871
238.068166	10335.127174	27.277888
238.377443	10350.790275	27.282906
238.394116	10363.966924	27.287924
238.803001	10381.518411	27.292941
238.899467	10394.281581	27.297959
238.959080	10411.003712	27.302976
239.099866	10429.260316	27.307994
239.120682	10448.697691	27.313012
239.677796	10480.011696	27.318029
239.684751	10494.866594	27.323047
240.243884	10508.239384	27.328064
240.134172	10521.091774	27.333082
240.823781	10541.160176	27.338100
241.341750	10556.209774	27.343117
241.233946	10574.016047	27.348135
241.699299	10599.095894	27.353152
241.856857	10612.054881	27.358170
242.260767	10624.381670	27.363188
242.904978	10633.210169	27.368205
242.906774	10657.525967	27.373223
242.853269	10652.096999	27.378240
242.879873	10669.373944	27.383258
243.084773	10681.570911	27.388276
243.725937	10702.916407	27.393293
243.556877	10719.999864	27.398311
244.106304	10724.994209	27.403328
244.019212	10739.241997	27.408346
244.465924	10760.327526	27.413364
244.628344	10777.258066	27.418381
244.838510	10789.198517	27.423399
245.207851	10804.138981	27.428416
245.738354	10821.532897	27.433434
245.484753	10824.979558	27.438452
245.976240	10841.887025	27.443469
246.017326	10859.297651	27.448487
246.300306	10878.801761	27.453504
246.690105	10886.849267	27.458522
246.916784	10909.200886	27.463540
247.158589	10915.206533	27.468557
247.146260	10943.383475	27.473575
247.589642	10941.403604	27.478592
247.754263	10962.710376	27.483610
247.865143	10980.672231	27.488628
248.320948	11003.060694	27.493645
248.465455	11026.726254	27.498663
248.853476	11043.261727	27.503680
249.320865	11052.326527	27.508698
249.261970	11064.520862	27.513716
249.652341	11083.206330	27.518733
249.547693	11100.895776	27.523751
250.039392	11121.892567	27.528768
250.485013	11142.407170	27.533786
250.434004	11157.442184	27.538804
251.003254	11181.243489	27.543821
250.911902	11190.525348	27.548839
251.165439	11210.091251	27.553856
251.755504	11220.722045	27.558874
252.253416	11232.301940	27.563892
252.297640	11248.146250	27.568909
252.608043	11270.377824	27.573927
252.906205	11286.709712	27.578944
253.305203	11291.153085	27.583962
253.526699	11305.056143	27.588980
253.735792	11327.294182	27.593997
253.732732	11331.797390	27.599015
253.942326	11344.688737	27.604032
254.136349	11363.474712	27.609050
254.051662	11385.098891	27.614068
254.664131	11398.653425	27.619085
254.624237	11425.689178	27.624103
254.873529	11431.719079	27.629120
255.436767	11455.587986	27.634138
255.839413	11490.616036	27.639156
255.590472	11506.541223	27.644173
256.272033	11526.131979	27.649191
256.503927	11527.377594	27.654208
256.715526	11543.540120	27.659226
256.831696	11572.970422	27.664244
257.305816	11582.309145	27.669261
257.388347	11617.826498	27.674279
257.980726	11629.003443	27.679296
258.114142	11647.480268	27.684314
258.117535	11666.252200	27.689332
258.874500	11684.400869	27.694349
258.843041	11697.560732	27.699367
259.279198	11710.514727	27.704384
259.404916	11720.425961	27.709402
259.336421	11734.055835	27.714420
259.875581	11756.040583	27.719437
260.459356	11769.678824	27.724455
259.966925	11790.505284	27.729472
260.825366	11804.706807	27.734490
260.953742	11823.639307	27.739508
261.409128	11838.371338	27.744525
261.631110	11856.673450	27.749543
261.745104	11859.652208	27.754560
262.179650	11881.404029	27.759578
262.255119	11904.945726	27.764596
262.252482	11910.317386	27.769613
262.658985	11923.967720	27.774631
262.534931	11937.019103	27.779648
262.725736	11956.696660	27.784666
262.920783	11974.952582	27.789684
263.421413	11999.558272	27.794701
263.682325	12015.962942	27.799719
264.210522	12035.294056	27.804736
264.790290	12045.203805	27.809754
264.900934	12067.511823	27.814772
264.622677	12080.849557	27.819789
265.140688	12103.867458	27.824807
265.030379	12122.806071	27.829824
265.748561	12142.189636	27.834842
265.980152	12157.759053	27.839860
266.406222	12186.854409	27.844877
266.721937	12200.437064	27.849895
266.972704	12215.529855	27.854912
267.385784	12222.680634	27.859930
267.510677	12233.397506	27.864948
267.644055	12263.520906	27.869965
268.115408	12269.459451	27.874983
268.062880	12291.591196	27.880000
268.371678	12312.377978	27.885018
268.890313	12328.392031	27.890036
268.804427	12347.481776	27.895053
269.467097	12368.146871	27.900071
269.557048	12393.973172	27.905088
269.612764	12407.385131	27.910106
270.018802	12434.194581	27.915124
270.382268	12450.075154	27.920141
270.664554	12462.482204	27.925159
271.010610	12487.722209	27.930176
271.349517	12507.787659	27.935194
271.384460	12532.148053	27.940212
271.503356	12550.157517	27.945229
271.653226	12562.923267	27.950247
271.811388	12584.567619	27.955264
272.745747	12617.796598	27.960282
272.745271	12638.960605	27.965300
272.910843	12651.136591	27.970317
273.265253	12672.942932	27.975335
273.388670	12689.186571	27.980352
273.899534	12713.068436	27.985370
274.231503	12747.876212	27.990388
274.347428	12751.931648	27.995405
274.388653	12779.777681	28.000423
274.438740	12792.682375	28.005440
275.070607	12820.644365	28.010458
275.330360	12840.043621	28.015476
276.106841	12859.529319	28.020493
276.309734	12876.458565	28.025511
276.327085	12899.843237	28.030528
276.723342	12923.133844	28.035546
277.044517	12933.962472	28.040564
276.971854	12955.914988	28.045581
277.896980	12980.701780	28.050599
278.216683	12998.329685	28.055616
278.442794	13001.780539	28.060634
278.715590	13030.626466	28.065652
279.360042	13042.219261	28.070669
279.665945	13054.926164	28.075687
279.392814	13066.530079	28.080704
279.782102	13073.814386	28.085722
280.091236	13096.537794	28.090740
280.256152	13113.034247	28.095757
280.800337	13112.254177	28.100775
280.436848	13123.749122	28.105792
280.899016	13139.990609	28.110810
281.023609	13163.952501	28.115828
281.494302	13173.848354	28.120845
281.691572	13180.635403	28.125863
281.587107	13208.413308	28.130880
281.979430	13237.240826	28.135898
282.668016	13256.885971	28.140916
282.352484	13269.611415	28.145933
282.929336	13283.327632	28.150951
283.108012	13315.321446	28.155968
283.784430	13335.344378	28.160986
283.808629	13350.811473	28.166004
284.119744	13369.372675	28.171021
284.530478	13393.062658	28.176039
284.340687	13409.807571	28.181056
285.096282	13437.542665	28.186074
285.501386	13460.084102	28.191092
285.795153	13469.692026	28.196109
285.955556	13486.881114	28.201127
286.362669	13508.190670	28.206144
286.755117	13535.932267	28.211162
286.810827	13539.312015	28.216180
287.079780	13564.312893	28.221197
287.746462	13581.365914	28.226215
287.366890	13598.036507	28.231232
288.035832	13619.772562	28.236250
287.983497	13637.014059	28.241268
288.590580	13651.079507	28.246285
288.884952	13674.680697	28.251303
288.951032	13692.844790	28.256320
289.404957	13707.853263	28.261338
290.066284	13748.472614	28.266356
289.876604	13761.134459	28.271373
290.267272	13776.187633	28.276391
290.628682	13800.754317	28.281408
290.530646	13813.951343	28.286426
290.984215	13839.953192	28.291444
291.146035	13876.359252	28.296461
291.478843	13890.723647	28.301479
291.752917	13913.841970	28.306496
292.545475	13931.699848	28.311514
292.817434	13953.915340	28.316532
293.080100	13974.389049	28.321549
293.157541	13992.946410	28.326567
293.655745	14013.793817	28.331584
294.038384	14029.514808	28.336602
294.352150	14047.517275	28.341620
294.278550	14064.269826	28.346637
294.428295	14088.664763	28.351655
294.651645	14112.659753	28.356672
295.283052	14125.629037	28.361690
295.081879	14148.853673	28.366708
295.908851	14177.949293	28.371725
296.197298	14191.597655	28.376743
296.361276	14221.128801	28.381760
296.689314	14246.977174	28.386778
297.238903	14262.662731	28.391796
297.418981	14285.890974	28.396813
298.119647	14306.315378	28.401831
298.241317	14316.673904	28.406848
298.546054	14330.705108	28.411866
299.180129	14361.691375	28.416884
299.183726	14373.641188	28.421901
299.339909	14376.395823	28.426919
299.708226	14405.374149	28.431936
299.864113	14430.122275	28.436954
300.341558	14442.231608	28.441972
300.346597	14460.285985	28.446989
300.775894	14470.890116	28.452007
300.779087	14493.277824	28.457024
301.008007	14504.008107	28.462042
301.391073	14525.110974	28.467060
301.633309	14547.732904	28.472077
302.114901	14563.113543	28.477095
302.413069	14585.802553	28.482112
302.476101	14600.228693	28.487130
302.644009	14617.847141	28.492148
303.074026	14653.773684	28.497165
303.598116	14675.337832	28.502183
303.632180	14699.331629	28.507200
303.506382	14708.544805	28.512218
304.522246	14743.236474	28.517236
304.484738	14758.853339	28.522253
304.763172	14777.357872	28.527271
304.754826	14805.704159	28.532288
305.324954	14836.003247	28.537306
305.853057	14858.542866	28.542324
305.894743	14885.700255	28.547341
306.186004	14904.237641	28.552359
306.578266	14940.356974	28.557376
307.193303	14961.749287	28.562394
307.409478	14988.140457	28.567412
307.698666	15019.390264	28.572429
308.059669	15035.421827	28.577447
308.352112	15065.085751	28.582464
308.929082	15084.507088	28.587482
308.891649	15109.602203	28.592500
309.061981	15126.879647	28.597517
309.682154	15141.225238	28.602535
309.328315	15173.975143	28.607552
309.950016	15192.757926	28.612570
310.697044	15216.223795	28.617588
311.023647	15254.195291	28.622605
311.433637	15274.571519	28.627623
311.915504	15297.801093	28.632640
312.011172	15323.797865	28.637658
312.460291	15343.182643	28.642676
312.887866	15367.560959	28.647693
312.999923	15381.111470	28.652711
313.237245	15396.471038	28.657728
313.675692	15412.591852	28.662746
313.917544	15440.723020	28.667764
314.504926	15465.679669	28.672781
314.674191	15479.537122	28.677799
315.291158	15507.609628	28.682816
315.396497	15522.187753	28.687834
315.873600	15540.412394	28.692852
316.191996	15558.646121	28.697869
316.170569	15573.130441	28.702887
316.477425	15591.546034	28.707904
316.642393	15614.427681	28.712922
317.480207	15631.023042	28.717940
317.518947	15652.095816	28.722957
317.802679	15668.177914	28.727975
318.074296	15693.721246	28.732992
318.156702	15718.210927	28.738010
318.580542	15735.316557	28.743028
319.037481	15757.928395	28.748045
319.165113	15793.418055	28.753063
319.188914	15809.480979	28.758080
319.936051	15831.946377	28.763098
320.337685	15852.592993	28.768116
320.289724	15876.481093	28.773133
320.601883	15906.348527	28.778151
321.225323	15930.933759	28.783168
321.075560	15937.542430	28.788186
321.508774	15964.381025	28.793204
321.410399	15990.642818	28.798221
322.200548	16011.645658	28.803239
322.347015	16040.076904	28.808256
322.681912	16061.719629	28.813274
323.531656	16085.116782	28.818292
323.253553	16103.542377	28.823309
323.766216	16121.534594	28.828327
324.062335	16153.956947	28.833344
324.563301	16173.729250	28.838362
324.697591	16193.770629	28.843380
325.064808	16224.198454	28.848397
325.517793	16247.686382	28.853415
325.933280	16281.318893	28.858432
325.974789	16299.211364	28.863450
326.617169	16317.631948	28.868468
326.675142	16340.695461	28.873485
326.907783	16373.371329	28.878503
327.235038	16394.045971	28.883520
327.361989	16420.851057	28.888538
327.807006	16444.662640	28.893556
328.282677	16484.009272	28.898573
329.119752	16506.467691	28.903591
329.520910	16525.324232	28.908608
329.214206	16558.125960	28.913626
329.960039	16576.644294	28.918644
329.990804	16591.197008	28.923661
330.528855	16621.380764	28.928679
330.895487	16641.228287	28.933696
331.045494	16679.505054	28.938714
331.659290	16696.692335	28.943732
331.573310	16727.049811	28.948749
332.123654	16744.856673	28.953767
332.578062	16772.384797	28.958784
332.626968	16802.670726	28.963802
332.976311	16827.565360	28.968820
333.422947	16856.727796	28.973837
333.894821	16872.661407	28.978855
334.069518	16905.015603	28.983872
334.267535	16933.967574	28.988890
334.952500	16962.742237	28.993908
335.199929	16990.479975	28.998925
335.581991	17005.814998	29.003943
336.257618	17023.093960	29.008960
336.228547	17054.362185	29.013978
336.881912	17079.351658	29.018996
336.911572	17102.966954	29.024013
337.335294	17108.623894	29.029031
337.618500	17148.295780	29.034048
338.316824	17175.849445	29.039066
338.482261	17195.053111	29.044084
338.764867	17218.376236	29.049101
338.946459	17232.239338	29.054119
339.253631	17260.801982	29.059136
339.436627	17288.556558	29.064154
339.791374	17317.440332	29.069172
340.406784	17346.656038	29.074189
340.371446	17375.045080	29.079207
341.095167	17393.997243	29.084224
341.281486	17424.954365	29.089242
341.681708	17441.240805	29.094260
342.240809	17474.773935	29.099277
342.342180	17500.103112	29.104295
342.299431	17518.695341	29.109312
342.739496	17545.847775	29.114330
343.174324	17572.558852	29.119348
343.447340	17604.589267	29.124365
343.608201	17632.524689	29.129383
343.996103	17650.342040	29.134400
343.961044	17677.316387	29.139418
344.527106	17709.143137	29.144436
344.790981	17746.614503	29.149453
345.230713	17767.595186	29.154471
345.845533	17800.810600	29.159488
345.913812	17829.177758	29.164506
346.305890	17853.211006	29.169524
346.517734	17884.720800	29.174541
346.838814	17913.749721	29.179559
347.698355	17935.757749	29.184576
348.008649	17969.665536	29.189594
348.433288	17998.798395	29.194612
348.595769	18024.573544	29.199629
349.032337	18054.683832	29.204647
349.429424	18074.490152	29.209664
349.593566	18107.650336	29.214682
350.261599	18134.224577	29.219700
350.484016	18160.653860	29.224717
350.993066	18186.880342	29.229735
351.076231	18208.384855	29.234752
351.265012	18242.362692	29.239770
352.053056	18265.904832	29.244788
352.401599	18289.263141	29.249805
352.717441	18316.587735	29.254823
353.279314	18340.790836	29.259840
353.360000	18373.680254	29.264858
353.321905	18402.014370	29.269876
354.052205	18437.878825	29.274893
354.358453	18461.490354	29.279911
355.009369	18486.797913	29.284928
355.033733	18529.147631	29.289946
355.546000	18542.972508	29.294964
355.737966	18572.300615	29.299981
356.019759	18604.154409	29.304999
356.519942	18625.025468	29.310016
356.700225	18654.816722	29.315034
357.589348	18687.327327	29.320052
357.601744	18713.796577	29.325069
357.802554	18742.997201	29.330087
358.234104	18774.196041	29.335104
358.413427	18799.059822	29.340122
358.785566	18834.336700	29.345140
359.297725	18864.025746	29.350157
359.289131	18891.585183	29.355175
360.090322	18926.580217	29.360192
360.294402	18959.950401	29.365210
360.836084	18990.329974	29.370228
361.339810	19025.548680	29.375245
362.061225	19053.985897	29.380263
362.268200	19070.866263	29.385280
362.332571	19103.639428	29.390298
362.491542	19125.114125	29.395316
363.023407	19155.659758	29.400333
363.339397	19185.935995	29.405351
364.232472	19214.245472	29.410368
364.285844	19246.540440	29.415386
364.440940	19261.426323	29.420404
365.017169	19294.239670	29.425421
365.047141	19320.454272	29.430439
365.427319	19361.732875	29.435456
366.246648	19381.057403	29.440474
366.443855	19408.920183	29.445492
366.706083	19435.408139	29.450509
367.259266	19460.593279	29.455527
367.599061	19485.022129	29.460544
367.484847	19516.156012	29.465562
367.867235	19544.034205	29.470580
368.143912	19576.951811	29.475597
368.782345	19596.494429	29.480615
369.177847	19616.346793	29.485632
369.406420	19657.485499	29.490650
369.661518	19683.684278	29.495668
370.400552	19701.568552	29.500685
370.463582	19731.891576	29.505703
371.231438	19761.504028	29.510720
371.381414	19787.713095	29.515738
371.813432	19823.178240	29.520756
372.034911	19842.116697	29.525773
372.460670	19874.689230	29.530791
373.126891	19913.618084	29.535808
373.109346	19940.883448	29.540826
373.545343	19968.614850	29.545844
374.257432	19992.891247	29.550861
374.194991	20024.738095	29.555879
374.937615	20049.180369	29.560896
374.844691	20080.760403	29.565914
375.443637	20102.464209	29.570932
375.593071	20134.259093	29.575949
376.040523	20172.275000	29.580967
376.487955	20199.417345	29.585984
376.904740	20237.968913	29.591002
377.280913	20274.460856	29.596020
377.724044	20297.149656	29.601037
378.140124	20324.056990	29.606055
378.823144	20361.758363	29.611072
378.869881	20389.134327	29.616090
379.359834	20425.880415	29.621108
379.799476	20457.270222	29.626125
380.193305	20485.868248	29.631143
380.644953	20509.307838	29.636160
380.978078	20544.985646	29.641178
381.408800	20572.383857	29.646196
381.888697	20595.427388	29.651213
382.020361	20625.305076	29.656231
382.584705	20652.455007	29.661248
382.875344	20681.688681	29.666266
383.418201	20709.638171	29.671284
383.623143	20734.272934	29.676301
383.397990	20774.019185	29.681319
384.272530	20805.764761	29.686336
384.819818	20843.273493	29.691354
384.724788	20873.920003	29.696372
385.558195	20901.445150	29.701389
385.888858	20939.923127	29.706407
386.483558	20974.044314	29.711424
386.879858	21002.225686	29.716442
387.183432	21034.080020	29.721460
387.598645	21064.905961	29.726477
387.614423	21096.824431	29.731495
388.290925	21125.366473	29.736512
388.776119	21156.263736	29.741530
389.030714	21180.739635	29.746548
389.603908	21212.071817	29.751565
389.517293	21250.293515	29.756583
390.106545	21281.629611	29.761600
390.589069	21306.101557	29.766618
391.022818	21342.693878	29.771636
391.572853	21376.247768	29.776653
391.532156	21405.066838	29.781671
391.839186	21429.812852	29.786688
392.243097	21468.488900	29.791706
392.438996	21500.739970	29.796724
393.476885	21539.468501	29.801741
393.810206	21575.659955	29.806759
394.006167	21599.437869	29.811776
394.496393	21630.151845	29.816794
394.674674	21653.749353	29.821812
395.052960	21679.880946	29.826829
395.180412	21720.559583	29.831847
395.663990	21748.090161	29.836864
396.266306	21775.178826	29.841882
396.453967	21807.425367	29.846900
396.951411	21834.852795	29.851917
397.288034	21873.445395	29.856935
397.693593	21904.141465	29.861952
398.030553	21941.634682	29.866970
398.285595	21971.665687	29.871988
399.098207	22013.495042	29.877005
398.964233	22043.005761	29.882023
399.658564	22076.228617	29.887040
400.411355	22107.521451	29.892058
400.478667	22154.788291	29.897076
401.497012	22182.589566	29.902093
401.547615	22211.029015	29.907111
401.807018	22246.481330	29.912128
402.177057	22273.291117	29.917146
402.687680	22309.936375	29.922164
403.178697	22341.043102	29.927181
403.541821	22378.691020	29.932199
404.020964	22409.995601	29.937216
404.373251	22435.917421	29.942234
404.136140	22476.623117	29.947252
405.069306	22519.148697	29.952269
405.002233	22554.463131	29.957287
406.088052	22589.123122	29.962304
406.460245	22619.351603	29.967322
406.728237	22654.771707	29.972340
407.112429	22704.903277	29.977357
407.456371	22735.749304	29.982375
407.930412	22773.209983	29.987392
408.507635	22797.460414	29.992410
408.740312	22845.271707	29.997428
409.110965	22874.521365	30.002445
409.536697	22910.106787	30.007463
409.746508	22943.053121	30.012480
410.459576	22978.928572	30.017498
410.706380	23016.905554	30.022516
411.305147	23056.331430	30.027533
411.604848	23102.654168	30.032551
412.258619	23129.509137	30.037568
412.452319	23161.706378	30.042586
413.082489	23207.933365	30.047604
413.446080	23235.693336	30.052621
413.585776	23269.687538	30.057639
413.682339	23316.282720	30.062656
414.471844	23348.570196	30.067674
414.781396	23394.689856	30.072692
415.324045	23427.313130	30.077709
415.542212	23465.832587	30.082727
416.277857	23500.498466	30.087744
416.921120	23534.698610	30.092762
417.410898	23573.927726	30.097780
417.793964	23615.221086	30.102797
418.138974	23648.684550	30.107815
418.674379	23676.114896	30.112832
419.403517	23712.469420	30.117850
419.335946	23744.917063	30.122868
420.050144	23767.257741	30.127885
420.188667	23799.325627	30.132903
420.972164	23826.767876	30.137920
421.153393	23852.016885	30.142938
421.685466	23888.269889	30.147956
421.812729	23910.096000	30.152973
422.424033	23936.939751	30.157991
422.689892	23962.542169	30.163008
423.430229	23997.302968	30.168026
423.462843	24032.395860	30.173044
424.052889	24054.225474	30.178061
423.984282	24089.170014	30.183079
424.412527	24119.373033	30.188096
425.168835	24154.542369	30.193114
425.550331	24189.802072	30.198132
425.711609	24224.337991	30.203149
426.331844	24265.684019	30.208167
426.286710	24299.727880	30.213184
427.200647	24329.968894	30.218202
427.313791	24366.332619	30.223220
427.784828	24396.415602	30.228237
428.382207	24444.938263	30.233255
428.746003	24485.414895	30.238272
429.337106	24514.373324	30.243290
429.619158	24566.073862	30.248308
429.963364	24596.265485	30.253325
430.156945	24637.306251	30.258343
430.983092	24682.330503	30.263360
431.531900	24712.370180	30.268378
432.070210	24753.129680	30.273396
432.580978	24797.148207	30.278413
432.883042	24822.114085	30.283431
433.335660	24858.008429	30.288448
433.658091	24890.643306	30.293466
433.786017	24925.937700	30.298484
434.591341	24967.881837	30.303501
434.828652	24998.571107	30.308519
434.738285	25046.406658	30.313536
435.443845	25091.709827	30.318554
435.996745	25139.078296	30.323572
436.107446	25182.269240	30.328589
436.924646	25223.611671	30.333607
437.205803	25271.130451	30.338624
438.105891	25306.904951	30.343642
438.398204	25344.323072	30.348660
438.679705	25375.524222	30.353677
439.375108	25421.897780	30.358695
440.095572	25465.057021	30.363712
440.340278	25493.609768	30.368730
440.804786	25538.958019	30.373748
441.198721	25566.539511	30.378765
441.439848	25607.391529	30.383783
441.759553	25657.717549	30.388800
442.747304	25689.977754	30.393818
443.113085	25733.610241	30.398836
443.338283	25772.272061	30.403853
444.031301	25806.316610	30.408871
444.357758	25851.927347	30.413888
444.879714	25882.636579	30.418906
445.482574	25919.027524	30.423924
445.495847	25960.472107	30.428941
446.413195	26004.644471	30.433959
446.409649	26037.534503	30.438976
447.252310	26060.173622	30.443994
447.377680	26105.525705	30.449012
447.885335	26143.221261	30.454029
448.192756	26180.227759	30.459047
448.734864	26222.272618	30.464064
449.116604	26260.999335	30.469082
449.399024	26304.532348	30.474100
450.017643	26344.347107	30.479117
450.849090	26376.594973	30.484135
451.024359	26416.826926	30.489152
451.718962	26438.762840	30.494170
452.060598	26478.248356	30.499188
452.185390	26507.415415	30.504205
453.291975	26543.722267	30.509223
453.330064	26576.018872	30.514240
453.616038	26605.818130	30.519258
454.190348	26640.679029	30.524276
454.361680	26670.369934	30.529293
455.148326	26707.656269	30.534311
454.835276	26744.407046	30.539328
455.700848	26787.698072	30.544346
456.286317	26833.883521	30.549364
456.674183	26874.740394	30.554381
457.211696	26915.529668	30.559399
457.702984	26947.888607	30.564416
457.861413	26993.325981	30.569434
458.300821	27032.847825	30.574452
458.592078	27071.375369	30.579469
459.310836	27110.815688	30.584487
459.658104	27164.769038	30.589504
460.292060	27198.825182	30.594522
461.017791	27245.539475	30.599540
461.194267	27290.873559	30.604557
461.865387	27337.147864	30.609575
461.964009	27369.619541	30.614592
462.696046	27417.015850	30.619610
462.853074	27462.694669	30.624628
463.355491	27508.382698	30.629645
464.348449	27558.734395	30.634663
464.452926	27592.779322	30.639680
465.181643	27628.414120	30.644698
465.183800	27676.462600	30.649716
465.740201	27727.079028	30.654733
466.461906	27765.609991	30.659751
466.588018	27820.648936	30.664768
467.210543	27854.695328	30.669786
467.842697	27912.543785	30.674804
468.143259	27954.554214	30.679821
468.775514	27991.216060	30.684839
469.212956	28050.789344	30.689856
469.877662	28087.888729	30.694874
469.963081	28130.280855	30.699892
470.472580	28172.556080	30.704909
470.878109	28211.352313	30.709927
471.392420	28263.499959	30.714944
471.913936	28313.238398	30.719962
472.465981	28366.183133	30.724980
472.971104	28418.724502	30.729997
473.580824	28445.650349	30.735015
473.691816	28486.812972	30.740032
474.025565	28532.517068	30.745050
475.109077	28582.029079	30.750068
475.311452	28632.361873	30.755085
476.083979	28662.934927	30.760103
476.387914	28716.437740	30.765120
477.069256	28765.943657	30.770138
477.447471	28803.917252	30.775156
478.097693	28853.763264	30.780173
478.385040	28892.250608	30.785191
478.640629	28938.770612	30.790208
478.882853	28983.105758	30.795226
479.992675	29024.612373	30.800244
480.524101	29080.071612	30.805261
480.763780	29115.147179	30.810279
481.417272	29161.049115	30.815296
481.837157	29200.957473	30.820314
482.292736	29237.604977	30.825332
482.613751	29280.746389	30.830349
483.230321	29313.317013	30.835367
483.532900	29358.844520	30.840384
483.827676	29394.487153	30.845402
484.447135	29439.927282	30.850420
484.785279	29487.592360	30.855437
484.949256	29526.270884	30.860455
485.416276	29571.969062	30.865472
486.126436	29619.607784	30.870490
486.511391	29661.918229	30.875508
486.970271	29715.766001	30.880525
487.542471	29756.985353	30.885543
487.820426	29800.577082	30.890560
488.278937	29856.024547	30.895578
488.978319	29894.177417	30.900596
489.360080	29951.457680	30.905613
489.883102	29997.002640	30.910631
490.260963	30047.949858	30.915648
490.582394	30098.002093	30.920666
491.252910	30154.700382	30.925684
491.673910	30216.848980	30.930701
492.592243	30263.584239	30.935719
493.018807	30316.111153	30.940736
493.317946	30361.483376	30.945754
493.713458	30412.062087	30.950772
494.550936	30461.136735	30.955789
495.046222	30502.413873	30.960807
495.845097	30567.222556	30.965824
496.369371	30603.444512	30.970842
496.955124	30656.181251	30.975860
497.289949	30705.607031	30.980877
497.737111	30746.095683	30.985895
498.095897	30803.091113	30.990912
498.479786	30855.942156	30.995930
498.871061	30897.021438	31.000948
499.313211	30962.968217	31.005965
500.182881	31006.412915	31.010983
500.881839	31059.859933	31.016000
501.246570	31100.905846	31.021018
502.025693	31146.571265	31.026036
502.043979	31205.435438	31.031053
502.672559	31251.181561	31.036071
503.357371	31303.588347	31.041088
504.364100	31348.687542	31.046106
504.760413	31396.000212	31.051124
504.838295	31441.080722	31.056141
505.477544	31490.789421	31.061159
505.838993	31529.206852	31.066176
506.261115	31584.683608	31.071194
507.120072	31620.481938	31.076212
507.407082	31678.805940	31.081229
507.671262	31723.017083	31.086247
508.294632	31771.293889	31.091264
508.578898	31823.113572	31.096282
509.258411	31880.592756	31.101300
509.771020	31928.653365	31.106317
510.267531	31989.202330	31.111335
510.752082	32040.466467	31.116352
510.713634	32085.749925	31.121370
511.825776	32135.000459	31.126388
511.925930	32190.181547	31.131405
512.641670	32251.291198	31.136423
513.386481	32301.187600	31.141440
513.876601	32352.685544	31.146458
514.436660	32402.718599	31.151476
514.827978	32459.207704	31.156493
515.259735	32510.455975	31.161511
515.771473	32560.079720	31.166528
516.596568	32603.914061	31.171546
517.190263	32642.613271	31.176564
517.167379	32696.835042	31.181581
517.467845	32737.280998	31.186599
518.046316	32789.720820	31.191616
518.602671	32840.760721	31.196634
519.260873	32897.013221	31.201652
519.552609	32949.782849	31.206669
519.987907	32998.686232	31.211687
520.879231	33051.728896	31.216704
521.585622	33116.395619	31.221722
521.716469	33164.841295	31.226740
521.968107	33219.394431	31.231757
522.985670	33260.171641	31.236775
523.165552	33315.754152	31.241792
523.500903	33376.869764	31.246810
524.239488	33437.593639	31.251828
524.539336	33506.940534	31.256845
525.234857	33559.307045	31.261863
525.703946	33614.579509	31.266880
526.417640	33675.820083	31.271898
527.120913	33733.698943	31.276916
527.480776	33790.373584	31.281933
528.591408	33839.419728	31.286951
528.872203	33895.462146	31.291968
529.179461	33956.862030	31.296986
529.801909	34008.419182	31.302004
530.193382	34069.597562	31.307021
530.745014	34120.514860	31.312039
531.526910	34175.031680	31.317056
531.880701	34228.869628	31.322074
532.774511	34288.414616	31.327092
533.204171	34346.730013	31.332109
533.521735	34394.390560	31.337127
534.081255	34457.193944	31.342144
534.811849	34514.059047	31.347162
535.294933	34572.676510	31.352180
535.723156	34622.520526	31.357197
536.331668	34680.783542	31.362215
537.055979	34736.518465	31.367232
537.407276	34796.010753	31.372250
538.144779	34852.369865	31.377268
538.757443	34912.200909	31.382285
539.198757	34965.666627	31.387303
540.010076	35001.908145	31.392320
540.298278	35069.959499	31.397338
540.943029	35113.631309	31.402356
541.483312	35178.956332	31.407373
542.090762	35230.809664	31.412391
542.416725	35285.704252	31.417408
542.966162	35337.231819	31.422426
543.626654	35397.012479	31.427444
544.100626	35448.400384	31.432461
544.930414	35500.036188	31.437479
545.310216	35557.622941	31.442496
545.738226	35615.442573	31.447514
546.261839	35660.563474	31.452532
546.991112	35718.456339	31.457549
547.382759	35778.077842	31.462567
548.265258	35832.753895	31.467584
548.648782	35887.413391	31.472602
549.490659	35935.697141	31.477620
550.004797	35992.075294	31.482637
550.259854	36043.947862	31.487655
551.201615	36084.919451	31.492672
551.362323	36147.195924	31.497690
551.700178	36188.414049	31.502708
552.565506	36250.472974	31.507725
553.106540	36296.793895	31.512743
553.745625	36339.887380	31.517760
553.973996	36392.852565	31.522778
554.107344	36441.065055	31.527796
554.548793	36489.406451	31.532813
554.991134	36550.969729	31.537831
555.724457	36600.403849	31.542848
556.041240	36659.780285	31.547866
556.762174	36709.355709	31.552884
557.425926	36767.862399	31.557901
557.955650	36837.475042	31.562919
558.679400	36892.577046	31.567936
558.910474	36954.294715	31.572954
559.630120	37012.255833	31.577972
560.246332	37075.209825	31.582989
560.585874	37136.019430	31.588007
561.393421	37204.426244	31.593024
561.509658	37255.153653	31.598042
562.138450	37324.252808	31.603060
562.737020	37379.002582	31.608077
563.357269	37451.480231	31.613095
564.032008	37507.135312	31.618112
564.541025	37586.055545	31.623130
565.562053	37643.952197	31.628148
565.755981	37714.828080	31.633165
566.421589	37775.904607	31.638183
567.027508	37832.918239	31.643200
567.917157	37893.416180	31.648218
568.585779	37946.980231	31.653236
568.971721	38007.822976	31.658253
569.699546	38074.581918	31.663271
570.328285	38122.840748	31.668288
570.350989	38181.046968	31.673306
571.111039	38248.092292	31.678324
571.464942	38316.870909	31.683341
572.127697	38380.909122	31.688359
572.821284	38435.583465	31.693376
573.220316	38512.488050	31.698394
573.652310	38578.978693	31.703412
574.108191	38640.134781	31.708429
574.647130	38713.280765	31.713447
575.496427	38782.116077	31.718464
576.369574	38851.485406	31.723482
576.991076	38923.050835	31.728500
577.769649	38982.683874	31.733517
578.121115	39037.931886	31.738535
578.930599	39098.123236	31.743552
579.215476	39170.602267	31.748570
580.011376	39226.034114	31.753588
580.843448	39288.005831	31.758605
581.563846	39352.139076	31.763623
582.073401	39405.010710	31.768640
582.234662	39471.388389	31.773658
583.219147	39525.621507	31.778676
583.929550	39581.472397	31.783693
584.460562	39646.312854	31.788711
585.225177	39705.633859	31.793728
585.520723	39761.512239	31.798746
586.096458	39804.217832	31.803764
586.508894	39870.879927	31.808781
587.101621	39934.908402	31.813799
587.482745	39982.748487	31.818816
588.255213	40057.468787	31.823834
589.114905	40118.717581	31.828852
589.773792	40171.118664	31.833869
590.292618	40231.858297	31.838887
591.084736	40281.234725	31.843904
591.680759	40343.417177	31.848922
592.320110	40391.824856	31.853940
592.591757	40443.439776	31.858957
592.943009	40504.535280	31.863975
593.639281	40544.782227	31.868992
593.874515	40609.210188	31.874010
594.764799	40662.271900	31.879028
595.400052	40715.468549	31.884045
595.552625	40777.601522	31.889063
596.381812	40831.552316	31.894080
596.801822	40891.474425	31.899098
597.590566	40944.653917	31.904116
598.125705	41003.894227	31.909133
598.832532	41072.588336	31.914151
599.206525	41133.884421	31.919168
599.618889	41198.608929	31.924186
600.122143	41261.611745	31.929204
600.828921	41326.347442	31.934221
601.244803	41393.475338	31.939239
601.929607	41458.651269	31.944256
602.521794	41528.579098	31.949274
602.850495	41608.022849	31.954292
603.315701	41674.258416	31.959309
604.129644	41746.979371	31.964327
605.404449	41818.660697	31.969344
605.647715	41890.851674	31.974362
606.402139	41962.374624	31.979380
607.164391	42027.894303	31.984397
607.401929	42102.971000	31.989415
608.492204	42162.190741	31.994432
608.623715	42234.318120	31.999450
609.435781	42298.622746	32.004468
610.682629	42366.913755	32.009485
610.948618	42436.332633	32.014503
611.297902	42501.867797	32.019520
611.924079	42565.829140	32.024538
612.739211	42640.108805	32.029556
613.650828	42699.566695	32.034573
613.988577	42761.815417	32.039591
614.535401	42844.518487	32.044608
615.197612	42899.676972	32.049626
615.691029	42967.866457	32.054644
616.553275	43043.133140	32.059661
616.961906	43114.119413	32.064679
618.108278	43171.448181	32.069696
618.546375	43240.962805	32.074714
619.327207	43303.940633	32.079732
620.040147	43373.652988	32.084749
620.614821	43435.208672	32.089767
621.136028	43498.657828	32.094784
621.501040	43561.290365	32.099802
622.108216	43626.668285	32.104820
622.798499	43700.983710	32.109837
623.240347	43768.380415	32.114855
624.094121	43838.154401	32.119872
624.667154	43904.303852	32.124890
625.375075	43971.235701	32.129908
626.012086	44039.140320	32.134925
626.480461	44110.525245	32.139943
627.089562	44186.664079	32.144960
627.706147	44252.984858	32.149978
628.143035	44312.319002	32.154996
628.750052	44375.915357	32.160013
629.356102	44460.101656	32.165031
630.266675	44519.887187	32.170048
630.557256	44596.355627	32.175066
631.239539	44663.154404	32.180084
632.484633	44732.465067	32.185101
633.010291	44807.018704	32.190119
633.417278	44872.368371	32.195136
634.273761	44925.028123	32.200154
634.430112	44979.252552	32.205172
635.441266	45036.240413	32.210189
635.819169	45104.884677	32.215207
636.798149	45165.989625	32.220224
637.367466	45226.576927	32.225242
637.814069	45287.537854	32.230260
638.797719	45349.401663	32.235277
639.126248	45412.823175	32.240295
639.450353	45472.658818	32.245312
640.637382	45543.935767	32.250330
640.873133	45610.250625	32.255348
641.840060	45659.067660	32.260365
642.116040	45730.475227	32.265383
642.842069	45803.349736	32.270400
643.659229	45863.134506	32.275418
643.944766	45934.085754	32.280436
644.618631	45997.454832	32.285453
645.235802	46083.094127	32.290471
645.767636	46148.162260	32.295488
646.807241	46212.910671	32.300506
647.401104	46288.148078	32.305524
648.301058	46358.631203	32.310541
648.489340	46436.070832	32.315559
649.277222	46506.647883	32.320576
649.885882	46584.471340	32.325594
650.855527	46653.249066	32.330612
651.794640	46723.923310	32.335629
652.201760	46788.664880	32.340647
652.854650	46857.809145	32.345664
653.783979	46930.490975	32.350682
653.895442	46994.767011	32.355700
654.508368	47069.877508	32.360717
655.131731	47133.124829	32.365735
655.882547	47214.426625	32.370752
656.414698	47285.141048	32.375770
657.048210	47363.482048	32.380788
657.996318	47433.170185	32.385805
658.897517	47508.559634	32.390823
659.111840	47583.474872	32.395840
659.922100	47656.778686	32.400858
660.596726	47734.184540	32.405876
661.105762	47800.981786	32.410893
661.673823	47880.960722	32.415911
662.463203	47961.310176	32.420928
663.248966	48029.386998	32.425946
664.156344	48108.124204	32.430964
664.697984	48172.133747	32.435981
665.397207	48251.201395	32.440999
666.122567	48324.318202	32.446016
667.052688	48394.265165	32.451034
667.329753	48465.086465	32.456052
667.986123	48535.532251	32.461069
668.603602	48620.934329	32.466087
669.223050	48690.608190	32.471104
669.675096	48766.793387	32.476122
669.990399	48840.703637	32.481140
670.996015	48919.883783	32.486157
671.730277	49003.548116	32.491175
672.725114	49072.354520	32.496192
673.365263	49155.553307	32.501210
673.836201	49231.287882	32.506228
674.590951	49302.948033	32.511245
675.206616	49378.514910	32.516263
675.998377	49457.224251	32.521280
676.865472	49529.164880	32.526298
677.401101	49598.196622	32.531316
678.014203	49669.044938	32.536333
678.348728	49738.640062	32.541351
679.642552	49814.924682	32.546368
680.094180	49873.986358	32.551386
680.287128	49953.537764	32.556404
681.188499	50015.509420	32.561421
681.536013	50095.378771	32.566439
682.396919	50174.389763	32.571456
683.177949	50245.030065	32.576474
683.664914	50325.220039	32.581492
684.520084	50399.639178	32.586509
685.133666	50478.582380	32.591527
685.927905	50557.143236	32.596544
686.668499	50630.625650	32.601562
687.066537	50713.051759	32.606580
687.339975	50794.624508	32.611597
688.239202	50870.177174	32.616615
688.607140	50951.691385	32.621632
689.948392	51030.845210	32.626650
690.430182	51121.637083	32.631668
690.705036	51200.819286	32.636685
691.099150	51290.897898	32.641703
692.118813	51389.617115	32.646720
693.014509	51475.068450	32.651738
693.670474	51575.465247	32.656756
694.649493	51655.133508	32.661773
694.948019	51741.672763	32.666791
696.074976	51825.943884	32.671808
696.603106	51919.313263	32.676826
697.297318	52012.517799	32.681844
697.816856	52090.051162	32.686861
698.775168	52183.082140	32.691879
699.265185	52274.199927	32.696896
700.450037	52361.336692	32.701914
701.062101	52444.716212	32.706932
702.036339	52530.165443	32.711949
702.624475	52612.726700	32.716967
703.171423	52706.248141	32.721984
703.942655	52787.231026	32.727002
704.796923	52878.445991	32.732020
705.409129	52970.578794	32.737037
706.295252	53054.506060	32.742055
706.778931	53142.685740	32.747072
707.445881	53226.363186	32.752090
708.190941	53312.756057	32.757108
708.967523	53408.604671	32.762125
709.764340	53494.661048	32.767143
710.104532	53583.503981	32.772160
711.123978	53667.431542	32.777178
711.682780	53756.601593	32.782196
712.266030	53850.931900	32.787213
713.268302	53945.209621	32.792231
713.898372	54030.844770	32.797248
714.530595	54118.827652	32.802266
715.234919	54213.184743	32.807284
715.961723	54293.686168	32.812301
717.110486	54382.867448	32.817319
717.563857	54480.460678	32.822336
718.321452	54561.388516	32.827354
718.824528	54641.514819	32.832372
719.738057	54733.607322	32.837389
720.490740	54828.022573	32.842407
720.730242	54914.949790	32.847424
721.761368	55007.170492	32.852442
722.596453	55103.890143	32.857460
723.464575	55191.814754	32.862477
724.387688	55272.725426	32.867495
724.789145	55362.647612	32.872512
726.027333	55427.745122	32.877530
726.198502	55515.362386	32.882548
727.146452	55598.535904	32.887565
727.629747	55670.441610	32.892583
728.462939	55743.976155	32.897600
729.325265	55827.246152	32.902618
729.373119	55911.821117	32.907636
730.040058	55993.761627	32.912653
731.032290	56081.720717	32.917671
731.429170	56179.114581	32.922688
732.469035	56263.845552	32.927706
732.834042	56359.137662	32.932724
733.283819	56451.562580	32.937741
734.570278	56543.363183	32.942759
735.084502	56641.829113	32.947776
736.314993	56726.107835	32.952794
736.570227	56816.798866	32.957812
737.549666	56915.186737	32.962829
738.061545	57013.641899	32.967847
738.616939	57119.242408	32.972864
739.648308	57201.743891	32.977882
740.384557	57311.607991	32.982900
740.608041	57396.951813	32.987917
741.848311	57495.427793	32.992935
742.607571	57591.036462	32.997952
743.334304	57686.922757	33.002970
743.896300	57783.214980	33.007988
745.304571	57888.109344	33.013005
746.164327	57988.912776	33.018023
746.505722	58092.658620	33.023040
747.274642	58179.071714	33.028058
748.148597	58270.158671	33.033076
748.686136	58371.204032	33.038093
749.550717	58465.394557	33.043111
750.538009	58566.882981	33.048128
751.458334	58662.014946	33.053146
752.099690	58759.463230	33.058164
752.545602	58858.005857	33.063181
753.537214	58941.019529	33.068199
754.136505	59043.880903	33.073216
754.982536	59144.115301	33.078234
755.537770	59241.351139	33.083252
756.777162	59337.068734	33.088269
757.506155	59431.341201	33.093287
758.289003	59527.320924	33.098304
759.125386	59621.577309	33.103322
759.575116	59714.021023	33.108340
760.199263	59819.989644	33.113357
761.080877	59905.112623	33.118375
761.930522	60002.691501	33.123392
763.056373	60094.518068	33.128410
763.756250	60193.437750	33.133428
764.291172	60298.314699	33.138445
765.176260	60379.102859	33.143463
766.214332	60488.193460	33.148480
766.569330	60579.623506	33.153498
767.714917	60671.942877	33.158516
767.857132	60768.002460	33.163533
768.876508	60861.310787	33.168551
769.666076	60960.687930	33.173568
770.575789	61055.356122	33.178586
771.608505	61160.633548	33.183604
771.970145	61252.963919	33.188621
772.628374	61352.432839	33.193639
773.625145	61443.803575	33.198656
774.213381	61542.094159	33.203674
774.946984	61631.582438	33.208692
776.004001	61729.502842	33.213709
776.682467	61819.855011	33.218727
777.186153	61917.767854	33.223744
777.743012	62000.739686	33.228762
778.506013	62093.681351	33.233780
779.348345	62188.889849	33.238797
780.225231	62284.086972	33.243815
780.615025	62378.936600	33.248832
781.550774	62472.283095	33.253850
782.294517	62579.745144	33.258868
783.282937	62681.915088	33.263885
784.182341	62773.312303	33.268903
784.563509	62875.989613	33.273920
785.409891	62970.023000	33.278938
786.380656	63074.064814	33.283956
787.019432	63175.645821	33.288973
787.869250	63282.568853	33.293991
788.754346	63386.321516	33.299008
789.170598	63487.944967	33.304026
789.854012	63594.680150	33.309044
790.753489	63700.160132	33.314061
791.883664	63804.300307	33.319079
792.679788	63904.504861	33.324096
793.500662	64007.143282	33.329114
794.140845	64112.399709	33.334132
794.872134	64218.269062	33.339149
795.847208	64327.101505	33.344167
796.844340	64436.032259	33.349184
797.701916	64536.976754	33.354202
798.336856	64645.882830	33.359220
799.043621	64754.056401	33.364237
800.044541	64857.163911	33.369255
800.614874	64960.972367	33.374272
801.578360	65070.297322	33.379290
802.603210	65183.513071	33.384308
803.071628	65298.038358	33.389325
804.170788	65396.124796	33.394343
805.033894	65506.252411	33.399360
805.854791	65621.407728	33.404378
807.043335	65720.158860	33.409396
807.427449	65822.201949	33.414413
808.286066	65926.317436	33.419431
809.154017	66041.815511	33.424448
809.813180	66143.133041	33.429466
810.874752	66252.530041	33.434484
811.721614	66359.586877	33.439501
812.344476	66454.554657	33.444519
813.441252	66572.114990	33.449536
813.892530	66679.349077	33.454554
814.966156	66778.419890	33.459572
815.528604	66886.080639	33.464589
816.667782	66991.840721	33.469607
817.720713	67101.002116	33.474624
818.346936	67211.180528	33.479642
819.261460	67302.737398	33.484660
819.619898	67412.838308	33.489677
820.853867	67508.910985	33.494695
821.313791	67615.204224	33.499712
822.204409	67719.834875	33.504730
823.005127	67823.144039	33.509748
823.893787	67946.302512	33.514765
825.262204	68041.374708	33.519783
825.960101	68145.613042	33.524800
826.633816	68249.716283	33.529818
827.694394	68355.291672	33.534836
828.385033	68458.183722	33.539853
829.129867	68562.144118	33.544871
829.961449	68660.019040	33.549888
830.673386	68761.110698	33.554906
831.536050	68854.783413	33.559924
832.120039	68952.090341	33.564941
832.896245	69056.440394	33.569959
834.008856	69138.291123	33.574976
834.449560	69241.459709	33.579994
835.659560	69336.738778	33.585012
836.142929	69453.312876	33.590029
837.110030	69554.506977	33.595047
837.708263	69658.564378	33.600064
838.357549	69768.262510	33.605082
839.542464	69869.980965	33.610100
840.313762	69976.912691	33.615117
841.358885	70075.785335	33.620135
841.869970	70188.900969	33.625152
842.436568	70294.447616	33.630170
843.440759	70398.799012	33.635188
844.354511	70520.059740	33.640205
845.516870	70626.616272	33.645223
846.231945	70735.294980	33.650240
846.979514	70845.957439	33.655258
847.410686	70960.102109	33.660276
848.036881	71077.420982	33.665293
849.317263	71187.089568	33.670311
850.159090	71302.868542	33.675328
850.763114	71421.192965	33.680346
852.296530	71538.688469	33.685364
852.675894	71660.316772	33.690381
853.611693	71769.345151	33.695399
854.444195	71886.217366	33.700416
855.473747	72012.533002	33.705434
856.664554	72124.157330	33.710452
857.613094	72242.520147	33.715469
858.138691	72354.186279	33.720487
859.572945	72464.494696	33.725504
859.790436	72575.044760	33.730522
861.342946	72690.997182	33.735540
862.043958	72807.324092	33.740557
862.605512	72923.521358	33.745575
863.580936	73037.551778	33.750592
864.480400	73140.372511	33.755610
866.108162	73247.576047	33.760628
866.545045	73376.156869	33.765645
867.090169	73477.590450	33.770663
867.853124	73594.582404	33.775680
868.975417	73712.025256	33.780698
870.066323	73821.417761	33.785716
870.523831	73933.240504	33.790733
871.291706	74042.139838	33.795751
872.732181	74159.965493	33.800768
873.229286	74288.781932	33.805786
874.173204	74404.545769	33.810804
875.091631	74515.057440	33.815821
876.140024	74617.670532	33.820839
876.913793	74732.005753	33.825856
877.628330	74858.333526	33.830874
878.814135	74963.941123	33.835892
879.840054	75088.789866	33.840909
880.214197	75193.081423	33.845927
881.444563	75305.346201	33.850944
882.028611	75430.354381	33.855962
883.245785	75538.974079	33.860980
884.106707	75648.232685	33.865997
884.946181	75762.612650	33.871015
886.045764	75883.184672	33.876032
886.702198	75995.694188	33.881050
887.800887	76104.765397	33.886068
888.301092	76227.041555	33.891085
889.535141	76336.776542	33.896103
890.157326	76439.235268	33.901120
890.829261	76543.105360	33.906138
891.816119	76638.869920	33.911156
892.363358	76755.985361	33.916173
893.356100	76858.463646	33.921191
894.329810	76968.102596	33.926208
895.101321	77088.401963	33.931226
895.764122	77192.541980	33.936244
896.899642	77306.210674	33.941261
897.584864	77429.502018	33.946279
898.533598	77536.752905	33.951296
899.208774	77662.973190	33.956314
900.110561	77783.837944	33.961332
900.870086	77911.414325	33.966349
901.743682	78028.990833	33.971367
902.900823	78148.018309	33.976384
903.492601	78279.182460	33.981402
904.368021	78401.726283	33.986420
905.366004	78530.357678	33.991437
906.429088	78664.921036	33.996455
907.582020	78787.701827	34.001472
908.179752	78925.886533	34.006490
909.385673	79046.202449	34.011508
910.061384	79174.443893	34.016525
910.935499	79303.098273	34.021543
911.766831	79427.148462	34.026560
912.702293	79558.518236	34.031578
913.819737	79694.813730	34.036596
914.346499	79834.559689	34.041613
915.231580	79958.502477	34.046631
916.337905	80086.579345	34.051648
917.039520	80237.360169	34.056666
918.091466	80368.145400	34.061684
918.931926	80516.524153	34.066701
919.782932	80651.548414	34.071719
921.293905	80786.761390	34.076736
921.844373	80913.928185	34.081754
922.787129	81049.712841	34.086772
923.988610	81194.997937	34.091789
924.644347	81322.935621	34.096807
925.830182	81463.891492	34.101824
926.567622	81605.374392	34.106842
927.882319	81741.154824	34.111860
929.074322	81872.824693	34.116877
929.685318	82010.832496	34.121895
931.176512	82138.529032	34.126912
931.369816	82277.046986	34.131930
932.306440	82402.867664	34.136948
933.645414	82546.440366	34.141965
934.605240	82683.003085	34.146983
935.792206	82815.387662	34.152000
936.550070	82955.619728	34.157018
937.345137	83078.145887	34.162036
938.324336	83213.795838	34.167053
939.404445	83342.195678	34.172071
940.435900	83469.133909	34.177088
941.199934	83610.381882	34.182106
942.235401	83738.765152	34.187124
942.787547	83866.578455	34.192141
943.969056	84008.700673	34.197159
944.983645	84143.652585	34.202176
945.889712	84283.918638	34.207194
946.660632	84410.154232	34.212212
948.065221	84536.962738	34.217229
948.638593	84679.056774	34.222247
950.051933	84810.300054	34.227264
950.683721	84949.826670	34.232282
951.507610	85071.533181	34.237300
952.681289	85189.485363	34.242317
953.618946	85317.333438	34.247335
954.750412	85437.700833	34.252352
955.269775	85563.727421	34.257370
956.447197	85682.834144	34.262388
957.502901	85806.572933	34.267405
957.639776	85933.459330	34.272423
958.823129	86063.071615	34.277440
960.286571	86199.077961	34.282458
960.575756	86325.460682	34.287476
961.996627	86457.293144	34.292493
962.220130	86594.775349	34.297511
963.612639	86729.236602	34.302528
964.442100	86871.706765	34.307546
965.699995	87002.236618	34.312564
966.980585	87128.632319	34.317581
967.706351	87277.064009	34.322599
968.610890	87406.016243	34.327616
969.683992	87546.652046	34.332634
970.269130	87685.983611	34.337652
971.646681	87816.549035	34.342669
972.308911	87960.647405	34.347687
973.010677	88102.142375	34.352704
974.016189	88249.141152	34.357722
975.391485	88385.564282	34.362740
976.388999	88532.692448	34.367757
976.766649	88677.662602	34.372775
978.149910	88816.240874	34.377792
979.166149	88965.471978	34.382810
979.818270	89110.946214	34.387828
980.560101	89251.844748	34.392845
981.814856	89417.237168	34.397863
983.110790	89546.682385	34.402880
984.176272	89701.016823	34.407898
985.001181	89852.360759	34.412916
986.524367	89998.615423	34.417933
987.091198	90149.760469	34.422951
988.425639	90297.212114	34.427968
989.289765	90443.622830	34.432986
990.316482	90585.775752	34.438004
991.320332	90724.270180	34.443021
992.363440	90877.486190	34.448039
993.842463	91028.416780	34.453056
994.648273	91169.504402	34.458074
995.619225	91309.400808	34.463092
996.507806	91447.789858	34.468109
997.600449	91595.653254	34.473127
999.063539	91735.145042	34.478144
999.845950	91892.145914	34.483162
1000.742294	92019.775837	34.488180
1002.121855	92165.695924	34.493197
1002.859593	92314.543616	34.498215
1004.076432	92452.112693	34.503232
1004.998367	92593.049317	34.508250
1006.002531	92727.218105	34.513268
1007.223185	92870.517428	34.518285
1007.618248	93008.306392	34.523303
1008.910488	93150.670556	34.528320
1010.341336	93288.235232	34.533338
1010.929494	93433.410700	34.538356
1012.296013	93553.583889	34.543373
1012.682603	93702.328516	34.548391
1013.870466	93846.854333	34.553408
1014.756370	93995.078564	34.558426
1015.694636	94144.714938	34.563444
1017.066745	94289.873093	34.568461
1017.765292	94436.024663	34.573479
1018.950158	94573.722308	34.578496
1019.974030	94712.459809	34.583514
1020.953751	94841.546066	34.588532
1021.893915	94968.116605	34.593549
1022.834486	95105.056287	34.598567
1023.915622	95228.994627	34.603584
1025.075391	95374.000954	34.608602
1025.910168	95509.437880	34.613620
1026.750792	95654.672937	34.618637
1027.782733	95788.533743	34.623655
1028.894254	95923.523502	34.628672
1030.116152	96071.096557	34.633690
1030.768925	96217.377714	34.638708
1032.020520	96359.724916	34.643725
1032.696696	96509.920704	34.648743
1033.744597	96656.192740	34.653760
1035.003764	96798.046361	34.658778
1035.910590	96952.340632	34.663796
1036.680160	97090.672118	34.668813
1037.329473	97246.503962	34.673831
1038.493093	97394.726156	34.678848
1039.708631	97560.738929	34.683866
1040.688415	97716.990378	34.688884
1041.951024	97870.967200	34.693901
1043.195502	98034.582003	34.698919
1043.946075	98192.925319	34.703936
1045.116699	98351.292393	34.708954
1045.900265	98508.123544	34.713972
1047.534917	98655.086210	34.718989
1048.637678	98826.751849	34.724007
1049.430652	98978.550997	34.729024
1050.575260	99140.462984	34.734042
1051.288299	99291.426745	34.739060
1052.531882	99453.096615	34.744077
1053.451025	99619.039686	34.749095
1054.960088	99769.779636	34.754112
1056.096596	99931.202435	34.759130
1057.136323	100094.530159	34.764148
1058.161963	100252.523594	34.769165
1059.093595	100412.028492	34.774183
1060.452299	100571.340531	34.779200
1061.658225	100731.095640	34.784218
1061.978178	100885.716208	34.789236
1063.283996	101051.136970	34.794253
1064.880268	101207.701826	34.799271
1065.691199	101368.434713	34.804288
1066.699771	101529.720643	34.809306
1067.560463	101685.502792	34.814324
1069.019416	101839.569189	34.819341
1070.306795	102017.904254	34.824359
1071.246336	102170.316578	34.829376
1072.416779	102328.550930	34.834394
1073.332464	102480.131637	34.839412
1074.456165	102641.189446	34.844429
1075.610673	102799.529974	34.849447
1076.890104	102963.772680	34.854464
1077.927007	103119.242389	34.859482
1078.590276	103276.280108	34.864500
1080.007161	103432.997717	34.869517
1080.673186	103599.152682	34.874535
1082.452093	103762.116624	34.879552
1083.421939	103909.067507	34.884570
1084.492264	104075.998366	34.889588
1085.654484	104233.659822	34.894605
1086.500306	104386.274476	34.899623
1087.535985	104546.886132	34.904640
1088.965357	104701.553669	34.909658
1090.002095	104856.638411	34.914676
1091.080004	105007.190828	34.919693
1091.879689	105151.980224	34.924711
1092.803093	105287.900483	34.929728
1094.363983	105434.511899	34.934746
1095.193293	105600.892096	34.939764
1096.391879	105741.842995	34.944781
1097.402240	105887.870530	34.949799
1098.043367	106033.893099	34.954816
1099.562776	106183.177023	34.959834
1100.326873	106341.189589	34.964852
1101.497160	106484.645957	34.969869
1102.120487	106646.955161	34.974887
1103.170851	106808.044380	34.979904
1104.712655	106970.655130	34.984922
1105.353851	107138.948947	34.989940
1106.677812	107302.685882	34.994957
1107.728244	107460.253000	34.999975
1108.998193	107631.887189	35.004992
1110.180379	107794.646895	35.010010
1110.930350	107966.820653	35.015028
1111.960343	108127.488086	35.020045
1113.182142	108297.040799	35.025063
1114.328921	108470.917559	35.030080
1115.582366	108640.403588	35.035098
1116.474253	108813.383578	35.040116
1117.725685	108994.664916	35.045133
1119.110402	109164.754309	35.050151
1119.731034	109339.465950	35.055168
1121.013722	109520.187146	35.060186
1121.911017	109701.324683	35.065204
1123.185891	109874.490897	35.070221
1124.385962	110048.963174	35.075239
1125.510536	110231.285267	35.080256
1126.743363	110409.495224	35.085274
1128.073083	110600.296398	35.090292
1129.282161	110777.028178	35.095309
1130.566329	110955.359660	35.100327
1131.829267	111133.606587	35.105344
1132.880113	111304.836513	35.110362
1134.117607	111472.093972	35.115380
1135.194696	111646.327035	35.120397
1136.456949	111826.441777	35.125415
1138.018522	111994.805009	35.130432
1138.987925	112172.494331	35.135450
1139.898547	112340.923048	35.140468
1141.103421	112513.757958	35.145485
1142.005493	112685.550422	35.150503
1142.929266	112861.246478	35.155520
1144.733554	113037.883548	35.160538
1145.613499	113218.711907	35.165556
1146.472382	113384.059053	35.170573
1147.919955	113566.474378	35.175591
1149.138025	113753.872796	35.180608
1150.413874	113916.455671	35.185626
1151.393300	114095.306984	35.190644
1152.447208	114264.089997	35.195661
1154.033830	114441.110391	35.200679
1154.986478	114618.953819	35.205696
1156.228406	114795.712810	35.210714
1157.460854	114970.381421	35.215732
1158.749367	115134.844816	35.220749
1159.845042	115312.199923	35.225767
1161.067637	115495.015192	35.230784
1162.230813	115659.944459	35.235802
1163.291541	115825.537351	35.240820
1164.332598	115997.805562	35.245837
1165.562472	116174.725230	35.250855
1166.511256	116353.541545	35.255872
1167.628990	116514.397600	35.260890
1168.796193	116696.301537	35.265908
1169.887263	116854.182558	35.270925
1171.136454	117014.906030	35.275943
1172.273340	117184.818204	35.280960
1173.307668	117347.859832	35.285978
1174.145082	117518.150173	35.290996
1175.455752	117695.305362	35.296013
1176.598046	117857.038516	35.301031
1177.571455	118037.469864	35.306048
1179.083808	118210.384753	35.311066
1180.118817	118388.486916	35.316084
1181.243531	118559.206277	35.321101
1182.601839	118735.800755	35.326119
1183.381155	118922.177605	35.331136
1184.512251	119102.538574	35.336154
1185.670052	119281.970240	35.341172
1186.886252	119469.334176	35.346189
1188.552433	119645.681700	35.351207
1189.364178	119839.935117	35.356224
1190.755540	120027.528043	35.361242
1192.112739	120218.958060	35.366260
1193.327467	120404.195709	35.371277
1194.162026	120586.842594	35.376295
1195.448543	120764.434360	35.381312
1196.959007	120948.309063	35.386330
1198.186193	121144.394057	35.391348
1199.442549	121321.295398	35.396365
1200.699339	121518.417823	35.401383
1201.994996	121705.780116	35.406400
1203.129152	121887.574318	35.411418
1204.628055	122070.187558	35.416436
1205.419262	122260.511064	35.421453
1206.723482	122436.407774	35.426471
1207.794592	122633.818561	35.431488
1209.555479	122822.001322	35.436506
1210.679766	123010.728635	35.441524
1211.897730	123194.482017	35.446541
1213.617209	123373.946023	35.451559
1214.303595	123563.239252	35.456576
1216.269158	123747.372900	35.461594
1217.078705	123931.662991	35.466612
1217.945302	124102.941722	35.471629
1219.442147	124287.341516	35.476647
1220.314414	124483.003815	35.481664
1221.544329	124670.517216	35.486682
1222.986674	124862.463830	35.491700
1224.224748	125046.603126	35.496717
1225.579231	125225.054182	35.501735
1226.539931	125428.445949	35.506752
1228.091441	125611.625307	35.511770
1229.403998	125808.176562	35.516788
1230.579819	125987.864157	35.521805
1231.915488	126171.777581	35.526823
1232.764104	126362.821947	35.531840
1234.213648	126559.050872	35.536858
1235.381769	126743.018453	35.541876
1236.435996	126936.266191	35.546893
1238.161832	127121.125048	35.551911
1239.012183	127313.924355	35.556928
1240.205966	127500.834695	35.561946
1241.235692	127689.370148	35.566964
1242.634291	127889.546387	35.571981
1244.071670	128076.281614	35.576999
1244.874179	128270.183941	35.582016
1246.417570	128456.155709	35.587034
1247.728938	128658.797959	35.592052
1248.857197	128856.420190	35.597069
1250.419137	129035.476882	35.602087
1251.287832	129221.824086	35.607104
1252.463693	129391.401579	35.612122
1253.879797	129586.000539	35.617140
1255.013321	129773.602863	35.622157
1256.500906	129937.995159	35.627175
1257.414312	130120.596369	35.632192
1258.430231	130315.870326	35.637210
1259.621637	130496.183842	35.642228
1260.810016	130692.891645	35.647245
1262.049343	130872.044616	35.652263
1262.775525	131068.623477	35.657280
1264.111401	131271.972158	35.662298
1265.206384	131469.675120	35.667316
1266.579851	131676.610620	35.672333
1268.028285	131879.056338	35.677351
1269.380933	132088.953471	35.682368
1270.946016	132294.351974	35.687386
1272.016783	132494.106238	35.692404
1273.042276	132692.777268	35.697421
1274.467587	132896.398673	35.702439
1275.271850	133113.758727	35.707456
1277.112295	133317.976913	35.712474
1278.131472	133534.074569	35.717492
1279.265598	133747.896638	35.722509
1280.991754	133953.163449	35.727527
1282.048950	134175.450536	35.732544
1283.754282	134375.951438	35.737562
1284.603216	134594.847127	35.742580
1286.016594	134816.066496	35.747597
1286.879162	135031.383789	35.752615
1288.484474	135252.587946	35.757632
1290.152965	135471.384981	35.762650
1291.673254	135682.402192	35.767668
1292.721351	135898.062560	35.772685
1294.034066	136107.743758	35.777703
1295.168909	136331.958131	35.782720
1296.874869	136555.119777	35.787738
1298.052845	136761.525713	35.792756
1299.295858	136994.076315	35.797773
1301.153704	137213.473853	35.802791
1302.148614	137432.779092	35.807808
1303.410963	137642.208678	35.812826
1304.712154	137846.696657	35.817844
1305.906047	138066.557486	35.822861
1307.802390	138290.002262	35.827879
1309.003062	138510.980864	35.832896
1310.334346	138712.599905	35.837914
1311.660497	138930.959311	35.842932
1312.834013	139150.358861	35.847949
1313.881845	139366.378031	35.852967
1315.493211	139581.561227	35.857984
1316.390955	139802.999392	35.863002
1318.191734	140011.657256	35.868020
1319.438733	140238.677460	35.873037
1320.540418	140461.977684	35.878055
1321.794283	140683.046906	35.883072
1323.231878	140900.331856	35.888090
1324.687202	141116.180923	35.893108
1325.955292	141346.731157	35.898125
1327.508203	141566.285442	35.903143
1328.722666	141784.916474	35.908160
1329.960026	142008.126447	35.913178
1331.156635	142224.198605	35.918196
1332.730510	142437.636313	35.923213
1334.087733	142660.043625	35.928231
1335.294393	142882.323211	35.933248
1336.419111	143107.967189	35.938266
1338.229711	143317.614952	35.943284
1338.925826	143530.661730	35.948301
1340.714784	143729.844007	35.953319
1341.962935	143934.226508	35.958336
1343.063540	144143.620819	35.963354
1344.598874	144336.220087	35.968372
1345.943181	144554.944554	35.973389
1347.266852	144765.893025	35.978407
1348.736745	144965.053991	35.983424
1349.968705	145180.409981	35.988442
1351.395223	145391.040344	35.993460
1352.545669	145609.342787	35.998477
1353.893170	145820.939205	36.003495
1355.256297	146034.019048	36.008512
1356.534545	146249.867295	36.013530
1357.938126	146466.877220	36.018548
1359.099449	146686.756390	36.023565
1360.501848	146912.627692	36.028583
1361.995928	147132.075887	36.033600
1363.182960	147362.577554	36.038618
1364.673580	147582.535889	36.043636
1365.894933	147819.761304	36.048653
1367.296854	148035.077193	36.053671
1368.872006	148264.252789	36.058688
1370.384795	148492.055617	36.063706
1371.409899	148730.128181	36.068724
1372.694441	148959.453812	36.073741
1374.269636	149171.853192	36.078759
1375.827018	149417.753269	36.083776
1376.606999	149645.053760	36.088794
1378.433382	149881.635162	36.093812
1379.674314	150120.365546	36.098829
1381.031448	150358.317194	36.103847
1382.746723	150593.345123	36.108864
1383.711042	150830.446397	36.113882
1385.463113	151062.538404	36.118900
1386.504454	151301.038632	36.123917
1388.112475	151539.730452	36.128935
1389.645834	151795.177908	36.133952
1391.044246	152024.346311	36.138970
1392.671993	152262.847752	36.143988
1393.773680	152506.027712	36.149005
1395.176493	152746.267393	36.154023
1396.662845	152986.495026	36.159040
1398.101725	153229.130274	36.164058
1399.132702	153459.237936	36.169076
1400.343256	153718.552885	36.174093
1401.965273	153966.963816	36.179111
1403.882557	154204.387220	36.184128
1404.941440	154461.418937	36.189146
1406.456716	154685.730629	36.194164
1407.976961	154932.422548	36.199181
1409.388275	155186.888849	36.204199
1410.778398	155437.259270	36.209216
1412.098582	155678.984054	36.214234
1413.736656	155926.067964	36.219252
1415.283698	156177.419858	36.224269
1417.041997	156420.500916	36.229287
1418.670345	156650.959369	36.234304
1419.614279	156906.420291	36.239322
1421.079187	157130.533408	36.244340
1422.566451	157383.588175	36.249357
1423.913389	157613.751631	36.254375
1425.534501	157851.490036	36.259392
1426.492620	158101.482288	36.264410
1427.941482	158343.159652	36.269428
1429.374132	158594.463420	36.274445
1430.788753	158838.788694	36.279463
1432.334892	159071.148145	36.284480
1433.673295	159302.601538	36.289498
1435.078570	159535.975020	36.294516
1436.182520	159766.997119	36.299533
1437.723764	160005.797398	36.304551
1439.138671	160239.349747	36.309568
1440.454168	160474.086513	36.314586
1441.909171	160705.437995	36.319604
1443.284013	160955.884373	36.324621
1444.450550	161186.724159	36.329639
1446.171384	161428.231287	36.334656
1447.492520	161682.802341	36.339674
1448.731732	161928.550948	36.344692
1450.075379	162176.467834	36.349709
1451.930034	162433.814920	36.354727
1453.401470	162669.957290	36.359744
1454.171912	162929.989838	36.364762
1455.972228	163191.017565	36.369780
1457.367560	163452.389032	36.374797
1458.572945	163705.640337	36.379815
1460.646321	163958.121944	36.384832
1461.719175	164223.673194	36.389850
1463.099201	164482.156368	36.394868
1465.224811	164750.008012	36.399885
1466.212209	165006.929525	36.404903
1468.244804	165264.056619	36.409920
1469.342589	165537.125439	36.414938
1471.246244	165784.307932	36.419956
1472.312618	166050.032418	36.424973
1473.950762	166310.589783	36.429991
1475.838287	166574.194393	36.435008
1476.769902	166845.466085	36.440026
1478.298404	167104.862794	36.445044
1479.758076	167374.022402	36.450061
1481.386308	167642.052027	36.455079
1483.131622	167903.373063	36.460096
1484.312766	168173.595060	36.465114
1485.959944	168445.598904	36.470132
1487.540141	168716.344556	36.475149
1489.298532	168988.675868	36.480167
1490.743392	169247.585586	36.485184
1491.895526	169513.474716	36.490202
1493.607785	169778.654980	36.495220
1495.405396	170048.482751	36.500237
1496.699756	170323.761254	36.505255
1498.238835	170583.029153	36.510272
1499.560472	170857.213384	36.515290
1501.253212	171124.534684	36.520308
1502.735873	171392.042183	36.525325
1504.094023	171670.375752	36.530343
1505.726819	171934.039694	36.535360
1507.167040	172209.822862	36.540378
1508.897512	172475.924030	36.545396
1510.885343	172746.011023	36.550413
1512.022824	173014.771801	36.555431
1513.566654	173278.162207	36.560448
1515.119839	173557.767231	36.565466
1516.082469	173828.196188	36.570484
1518.048637	174095.675447	36.575501
1519.281495	174375.828713	36.580519
1520.964119	174646.528698	36.585536
1522.518067	174912.246682	36.590554
1524.330392	175181.671050	36.595572
1525.597257	175441.721534	36.600589
1527.405588	175729.535307	36.605607
1528.984512	175994.960846	36.610624
1530.098303	176251.888678	36.615642
1531.671380	176532.504028	36.620660
1533.499544	176794.134398	36.625677
1534.680592	177058.355753	36.630695
1536.082228	177304.079838	36.635712
1537.871455	177564.398044	36.640730
1539.255368	177815.027999	36.645748
1540.831554	178070.631832	36.650765
1542.306421	178335.014325	36.655783
1543.867542	178588.488676	36.660800
1545.214438	178856.803966	36.665818
1546.672246	179118.753352	36.670836
1548.467725	179378.415682	36.675853
1549.413999	179643.164213	36.680871
1551.192581	179906.945141	36.685888
1552.647594	180185.787563	36.690906
1553.836259	180463.047067	36.695924
1555.785957	180719.920771	36.700941
1557.285048	181002.035126	36.705959
1558.882766	181277.810790	36.710976
1560.619594	181561.946891	36.715994
1562.182413	181847.254011	36.721012
1563.956314	182114.191390	36.726029
1565.284994	182396.844600	36.731047
1566.770471	182670.584653	36.736064
1568.719434	182952.050296	36.741082
1570.124597	183232.636722	36.746100
1571.879700	183513.626368	36.751117
1573.468220	183800.738591	36.756135
1575.331915	184075.769549	36.761152
1576.630154	184361.735091	36.766170
1578.326520	184653.455505	36.771188
1579.755077	184992.130699	36.776205
1581.312771	185283.722245	36.781223
1583.316644	185572.044497	36.786240
1585.021484	185856.426676	36.791258
1586.302019	186133.129248	36.796276
1587.968402	186417.341186	36.801293
1589.400512	186713.731502	36.806311
1591.434230	186986.508528	36.811328
1592.911526	187280.074005	36.816346
1594.691341	187562.950480	36.821364
1596.216787	187842.159143	36.826381
1597.573671	188142.171937	36.831399
1599.236148	188417.601453	36.836416
1601.112471	188718.347316	36.841434
1602.372495	189010.021043	36.846452
1604.108561	189296.972812	36.851469
1605.314336	189598.054570	36.856487
1607.293446	189876.968724	36.861504
1608.907114	190166.583453	36.866522
1610.399675	190466.555786	36.871540
1611.978056	190749.649602	36.876557
1613.696333	191056.852624	36.881575
1615.399527	191349.859913	36.886592
1617.033137	191637.239880	36.891610
1618.487906	191925.004125	36.896628
1620.159538	192231.658622	36.901645
1621.939640	192524.428094	36.906663
1623.638609	192823.027738	36.911680
1625.117002	193125.294936	36.916698
1626.729255	193420.226436	36.921716
1628.600568	193703.128805	36.926733
1630.067209	194008.295639	36.931751
1631.739580	194304.642208	36.936768
1633.244340	194604.749645	36.941786
1634.683857	194898.289054	36.946804
1636.557758	195202.048639	36.951821
1638.018092	195501.428395	36.956839
1639.849243	195794.629039	36.961856
1641.617338	196091.548782	36.966874
1642.575502	196377.546260	36.971892
1644.216576	196651.803537	36.976909
1645.604590	196939.894008	36.981927
1647.329852	197228.618121	36.986944
1648.779661	197513.016825	36.991962
1650.290433	197804.417418	36.996980
1651.904672	198104.464402	37.001997
1653.608624	198397.131412	37.007015
1655.149398	198692.847347	37.012032
1657.064069	199011.214674	37.017050
1658.542328	199307.856041	37.022068
1660.325059	199597.871192	37.027085
1662.011599	199911.729081	37.032103
1663.430329	200215.849672	37.037120
1665.426859	200519.855005	37.042138
1666.959790	200840.089269	37.047156
1668.894545	201131.048645	37.052173
1670.300125	201455.114352	37.057191
1671.850057	201741.003725	37.062208
1673.935085	202065.243676	37.067226
1675.510299	202383.416613	37.072244
1676.968077	202698.915831	37.077261
1678.772893	203022.744131	37.082279
1680.551011	203338.346741	37.087296
1682.144668	203649.076046	37.092314
1683.862169	203982.928320	37.097332
1685.727289	204287.621154	37.102349
1687.036929	204613.688907	37.107367
1688.826015	204943.746616	37.112384
1690.575366	205261.033457	37.117402
1692.103547	205595.095903	37.122420
1694.494879	205920.386815	37.127437
1695.983898	206242.720275	37.132455
1697.825104	206570.918003	37.137472
1699.627750	206892.187231	37.142490
1701.460392	207223.359428	37.147508
1702.572718	207539.809418	37.152525
1704.282956	207862.288433	37.157543
1706.466219	208191.781354	37.162560
1708.403239	208519.611249	37.167578
1710.021105	208854.020166	37.172596
1711.743057	209179.953952	37.177613
1713.504998	209503.570197	37.182631
1714.887341	209835.603952	37.187648
1716.856206	210160.738233	37.192666
1718.552500	210485.940964	37.197684
1720.722835	210812.746523	37.202701
1722.492255	211145.737436	37.207719
1724.241466	211468.291058	37.212736
1725.989197	211790.388001	37.217754
1727.718881	212114.113939	37.222772
1729.454768	212443.580452	37.227789
1731.143852	212767.923103	37.232807
1732.989997	213087.414810	37.237824
1734.509536	213414.502816	37.242842
1736.249062	213752.785132	37.247860
1738.029657	214074.955399	37.252877
1740.114945	214407.570007	37.257895
1741.700507	214729.542733	37.262912
1743.598700	215052.991029	37.267930
1745.236626	215378.563426	37.272948
1746.674433	215696.368430	37.277965
1748.658749	216021.074199	37.282983
1750.495175	216350.020389	37.288000
1752.472495	216668.529185	37.293018
1754.029947	216998.637259	37.298036
1756.113994	217323.328332	37.303053
1757.614299	217647.018591	37.308071
1759.117536	217948.048289	37.313088
1760.428587	218251.724830	37.318106
1762.518668	218561.910052	37.323124
1763.937015	218858.965087	37.328141
1765.810096	219179.625603	37.333159
1767.408063	219497.534886	37.338176
1769.412873	219801.129006	37.343194
1770.829753	220121.937553	37.348212
1772.484828	220438.314060	37.353229
1773.968830	220762.110028	37.358247
1775.801345	221092.507432	37.363264
1777.606993	221417.574304	37.368282
1778.873411	221756.011974	37.373300
1780.544935	222089.686600	37.378317
1782.820798	222423.952654	37.383335
1784.264881	222768.662999	37.388352
1786.031393	223116.523874	37.393370
1787.468344	223464.766638	37.398388
1789.403475	223813.261752	37.403405
1791.140737	224164.937980	37.408423
1792.789549	224524.859006	37.413440
1794.833179	224870.898451	37.418458
1796.804386	225234.122404	37.423476
1798.246890	225598.191215	37.428493
1799.981321	225953.983410	37.433511
1802.089345	226312.486169	37.438528
1804.217279	226672.637046	37.443546
1805.793202	227041.384624	37.448564
1807.537907	227405.685424	37.453581
1809.278122	227775.982218	37.458599
1810.862643	228151.358700	37.463616
1812.940362	228513.778051	37.468634
1814.645204	228896.248631	37.473652
1816.448317	229263.867747	37.478669
1818.677449	229637.288397	37.483687
1820.732940	230018.027024	37.488704
1822.341270	230377.064222	37.493722
1824.322163	230755.197572	37.498740
1826.269080	231123.225262	37.503757
1828.397253	231495.568475	37.508775
1830.091724	231856.801603	37.513792
1832.349989	232238.752124	37.518810
1834.369230	232608.596725	37.523828
1836.043843	232972.982361	37.528845
1837.902688	233337.034072	37.533863
1839.745872	233714.323387	37.538880
1842.021508	234074.727392	37.543898
1843.474873	234434.243632	37.548916
1845.416621	234804.835432	37.553933
1847.170108	235167.479583	37.558951
1849.428687	235536.293705	37.563968
1851.589249	235898.365430	37.568986
1853.215334	236266.490319	37.574004
1854.934524	236628.833639	37.579021
1857.173001	236976.767672	37.584039
1858.937293	237349.112241	37.589056
1860.778826	237715.042605	37.594074
1863.271005	238069.312122	37.599092
1864.771654	238420.510147	37.604109
1866.415931	238786.165307	37.609127
1868.624743	239139.334786	37.614144
1870.828418	239485.137643	37.619162
1872.481780	239848.706980	37.624180
1874.507636	240204.520332	37.629197
1876.699465	240541.788199	37.634215
1878.343998	240901.115160	37.639232
1880.320918	241243.572636	37.644250
1881.756959	241578.391695	37.649268
1884.259480	241909.105931	37.654285
1885.844851	242244.459597	37.659303
1887.310623	242578.180304	37.664320
1889.087273	242899.226545	37.669338
1890.897101	243239.421076	37.674356
1892.740990	243568.940488	37.679373
1894.433117	243907.196394	37.684391
1896.033727	244254.560360	37.689408
1898.084594	244591.107874	37.694426
1899.508428	244943.299533	37.699444
1901.253010	245295.923061	37.704461
1903.231839	245646.731130	37.709479
1904.702402	246020.378981	37.714496
1906.612640	246374.625869	37.719514
1908.199483	246743.707057	37.724532
1909.994446	247117.479849	37.729549
1912.225771	247494.485947	37.734567
1914.457986	247877.968771	37.739584
1916.195734	248243.263792	37.744602
1918.193207	248620.151720	37.749620
1919.603088	249004.040212	37.754637
1921.692437	249391.962104	37.759655
1923.542526	249783.553062	37.764672
1925.357575	250168.848847	37.769690
1927.150330	250561.640836	37.774708
1929.232786	250946.257887	37.779725
1931.413368	251350.113353	37.784743
1932.979603	251748.780307	37.789760
1935.262846	252150.331459	37.794778
1937.162676	252551.966944	37.799796
1938.794002	252947.496151	37.804813
1941.114913	253357.623948	37.809831
1943.032868	253757.678413	37.814848
1944.744212	254160.380445	37.819866
1946.795702	254571.080359	37.824884
1948.949786	254983.464900	37.829901
1950.988791	255391.598796	37.834919
1952.930761	255810.770765	37.839936
1955.093978	256214.539129	37.844954
1957.069933	256628.013353	37.849972
1958.835313	257031.739845	37.854989
1961.247449	257438.284975	37.860007
1962.977805	257851.260275	37.865024
1965.063035	258256.228268	37.870042
1967.465237	258676.766723	37.875060
1969.211178	259082.013691	37.880077
1971.345959	259489.509900	37.885095
1973.536199	259904.031941	37.890112
1975.175518	260314.066675	37.895130
1977.349828	260724.702065	37.900148
1979.487137	261136.408583	37.905165
1981.702162	261535.680854	37.910183
1983.500932	261940.935017	37.915200
1985.426979	262347.767979	37.920218
1987.914080	262756.696030	37.925236
1989.585962	263169.255246	37.930253
1991.706312	263567.239583	37.935271
1993.826487	263979.446145	37.940288
1996.057246	264374.387646	37.945306
1998.155267	264770.973973	37.950324
2000.387252	265175.665543	37.955341
2002.258471	265578.507031	37.960359
2003.708414	265967.037030	37.965376
2005.863217	266371.177125	37.970394
2008.023687	266768.355434	37.975412
2010.085077	267170.246390	37.980429
2012.178265	267562.580867	37.985447
2013.806685	267956.281786	37.990464
2015.905063	268342.643636	37.995482
2018.376549	268712.385895	38.000500
2019.573319	269097.412624	38.005517
2021.937965	269460.209558	38.010535
2023.428044	269854.762306	38.015552
2025.501828	270240.434389	38.020570
2027.730164	270623.744064	38.025588
2029.535653	271012.629541	38.030605
2031.790532	271392.198332	38.035623
2033.303826	271786.281828	38.040640
2035.364623	272192.544764	38.045658
2037.175113	272579.365367	38.050676
2038.871944	272990.506962	38.055693
2041.380919	273390.446471	38.060711
2043.099104	273807.345876	38.065728
2045.208640	274218.747105	38.070746
2047.519822	274624.349746	38.075764
2049.647685	275032.899664	38.080781
2051.342954	275442.658061	38.085799
2053.659027	275861.536063	38.090816
2055.812195	276278.380301	38.095834
2057.819363	276688.743868	38.100852
2060.066864	277110.571981	38.105869
2062.421398	277533.549285	38.110887
2064.155105	277951.364570	38.115904
2066.424260	278381.461350	38.120922
2068.478387	278796.225281	38.125940
2070.286973	279210.441286	38.130957
2072.931639	279641.894328	38.135975
2074.888048	280078.556916	38.140992
2077.178244	280485.859345	38.146010
2079.345367	280916.414721	38.151028
2081.168935	281344.532678	38.156045
2083.094654	281766.715295	38.161063
2085.304583	282196.062879	38.166080
2087.434968	282630.295958	38.171098
2089.596453	283055.963842	38.176116
2091.573438	283499.382725	38.181133
2093.700352	283922.130519	38.186151
2095.775263	284355.599826	38.191168
2098.008748	284786.553082	38.196186
2100.258487	285229.562721	38.201204
2102.275706	285679.614252	38.206221
2104.621461	286105.285294	38.211239
2106.711410	286546.965486	38.216256
2108.876085	286981.419660	38.221274
2110.997939	287416.436304	38.226292
2113.075171	287861.664595	38.231309
2115.347630	288289.872229	38.236327
2117.612004	288730.418599	38.241344
2119.767617	289165.545207	38.246362
2121.789460	289591.244242	38.251380
2123.733145	290031.120856	38.256397
2126.142687	290463.329644	38.261415
2127.759032	290905.815822	38.266432
2129.839629	291349.901992	38.271450
2132.134954	291793.316615	38.276468
2134.263900	292234.595900	38.281485
2136.531693	292669.223484	38.286503
2138.475208	293122.737897	38.291520
2140.867053	293578.641538	38.296538
2142.817370	294013.029791	38.301556
2144.639621	294463.277765	38.306573
2147.363053	294905.815388	38.311591
2149.695641	295347.776092	38.316608
2151.335720	295784.738668	38.321626
2153.777399	296225.177693	38.326644
2155.583815	296670.155670	38.331661
2157.786574	297088.436114	38.336679
2159.933958	297512.916779	38.341696
2161.834738	297930.095795	38.346714
2163.998061	298346.138975	38.351732
2166.323627	298777.944567	38.356749
2168.401593	299199.249890	38.361767
2170.828568	299625.473227	38.366784
2172.640068	300051.129485	38.371802
2174.926315	300471.453143	38.376820
2176.414754	300920.381785	38.381837
2178.921732	301353.687219	38.386855
2181.126507	301791.428184	38.391872
2183.150018	302240.719005	38.396890
2185.364811	302668.043057	38.401908
2186.970996	303138.461461	38.406925
2188.954701	303586.223919	38.411943
2191.367130	304034.753154	38.416960
2193.683473	304501.291197	38.421978
2196.026841	304962.693146	38.426996
2197.438872	305429.922675	38.432013
2200.253673	305884.591896	38.437031
2202.322505	306371.661725	38.442048
2204.648703	306834.343896	38.447066
2207.083495	307301.700680	38.452084
2209.403118	307774.629947	38.457101
2211.684341	308247.027658	38.462119
2214.094942	308711.506648	38.467136
2215.973683	309191.242979	38.472154
2218.458092	309672.098153	38.477172
2220.948785	310142.617211	38.482189
2223.483785	310621.449838	38.487207
2225.712811	311077.101744	38.492224
2227.420487	311562.374255	38.497242
2230.118102	312043.502150	38.502260
2232.315769	312526.581479	38.507277
2235.022795	313005.033080	38.512295
2237.530855	313472.851324	38.517312
2239.366664	313950.312739	38.522330
2242.062379	314426.086531	38.527348
2244.403403	314892.596725	38.532365
2246.562974	315373.520323	38.537383
2248.855424	315842.591605	38.542400
2250.958347	316301.561698	38.547418
2253.900496	316778.261948	38.552436
2256.220875	317253.074894	38.557453
2258.227336	317707.502963	38.562471
2260.798992	318181.556053	38.567488
2262.583700	318652.732642	38.572506
2265.192506	319116.187593	38.577524
2267.202659	319593.713655	38.582541
2269.531193	320068.139496	38.587559
2272.200054	320541.441074	38.592576
2274.365449	321016.161078	38.597594
2276.626457	321483.527367	38.602612
2278.597278	321951.314519	38.607629
2281.165991	322421.464295	38.612647
2283.571350	322884.478758	38.617664
2285.701692	323366.434858	38.622682
2288.124195	323822.534433	38.627700
2290.439420	324300.771528	38.632717
2292.867089	324770.891392	38.637735
2295.430778	325239.386079	38.642752
2297.532813	325701.680535	38.647770
2300.066205	326171.209500	38.652788
2301.631955	326632.536944	38.657805
2304.129935	327091.683514	38.662823
2306.219164	327558.170388	38.667840
2308.618047	328038.709767	38.672858
2310.863332	328477.405289	38.677876
2313.077985	328926.375847	38.682893
2315.442251	329369.913979	38.687911
2317.245608	329815.742022	38.692928
2319.700340	330272.701887	38.697946
2321.827639	330719.661266	38.702964
2323.571352	331174.590667	38.707981
2325.918410	331639.846921	38.712999
2328.409286	332097.007810	38.718016
2330.394848	332575.856034	38.723034
2333.031105	333046.960672	38.728052
2335.330198	333521.866586	38.733069
2337.115295	334006.790892	38.738087
2339.789109	334482.589986	38.743104
2341.721674	334970.776419	38.748122
2343.890620	335465.641527	38.753140
2346.654564	335966.038177	38.758157
2348.360421	336452.185853	38.763175
2350.778460	336953.536305	38.768192
2352.953225	337465.977024	38.773210
2355.271382	337963.854175	38.778228
2357.812555	338482.640422	38.783245
2360.304706	339003.050135	38.788263
2362.884226	339511.923593	38.793280
2365.035798	340034.273811	38.798298
2367.464735	340551.500400	38.803316
2369.635178	341077.763485	38.808333
2372.094189	341602.477192	38.813351
2374.800583	342115.858415	38.818368
2377.304860	342654.472743	38.823386
2379.786102	343187.300037	38.828404
2382.122691	343712.635039	38.833421
2384.396244	344232.113695	38.838439
2387.290124	344761.250897	38.843456
2389.553712	345309.447193	38.848474
2392.249769	345821.963139	38.853492
2394.593612	346355.193552	38.858509
2397.126940	346888.639442	38.863527
2399.454682	347424.340455	38.868544
2401.732433	347948.858120	38.873562
2404.377609	348481.272065	38.878580
2406.891723	349011.010140	38.883597
2409.474179	349540.906478	38.888615
2412.141057	350070.831740	38.893632
2414.205935	350605.482552	38.898650
2416.298528	351131.930622	38.903668
2419.284036	351667.129830	38.908685
2421.857573	352206.567974	38.913703
2424.191009	352735.436816	38.918720
2426.611968	353267.655162	38.923738
2429.233405	353805.005177	38.928756
2431.778512	354334.067817	38.933773
2434.277018	354873.294938	38.938791
2436.575720	355392.313636	38.943808
2439.011685	355932.090032	38.948826
2441.228244	356457.948594	38.953844
2444.139154	356994.260610	38.958861
2446.484877	357531.184051	38.963879
2449.117689	358059.358426	38.968896
2451.362497	358579.193932	38.973914
2453.828215	359120.481410	38.978932
2455.923544	359650.207843	38.983949
2458.284728	360186.828612	38.988967
2461.124653	360713.276835	38.993984
2463.218820	361257.625738	38.999002
2465.738861	361781.519865	39.004020
2468.749591	362319.876410	39.009037
2470.817483	362860.677061	39.014055
2473.413045	363367.093876	39.019072
2476.032047	363875.196372	39.024090
2478.803418	364382.581941	39.029108
2480.942314	364879.464074	39.034125
2482.786617	365376.738601	39.039143
2485.369097	365885.419997	39.044160
2487.963237	366395.104293	39.049178
2490.290611	366910.143031	39.054196
2492.762974	367435.767792	39.059213
2494.562612	367955.076907	39.064231
2497.336875	368471.107252	39.069248
2499.835411	369006.936361	39.074266
2502.164519	369536.142912	39.079284
2504.598775	370072.493951	39.084301
2506.925025	370615.338236	39.089319
2509.142876	371161.989602	39.094336
2511.533900	371707.919035	39.099354
2514.111552	372262.600406	39.104372
2516.867918	372815.899858	39.109389
2519.120069	373381.681586	39.114407
2521.712817	373941.039209	39.119424
2524.372613	374500.628233	39.124442
2526.717497	375078.622308	39.129460
2529.498138	375646.123755	39.134477
2531.769590	376220.406194	39.139495
2534.736392	376789.070431	39.144512
2536.988689	377372.349618	39.149530
2539.344720	377960.438146	39.154548
2542.291301	378543.811062	39.159565
2544.765691	379131.804442	39.164583
2547.390139	379703.879446	39.169600
2550.041580	380298.278178	39.174618
2552.610920	380880.239868	39.179636
2555.263668	381472.180125	39.184653
2558.048756	382058.539460	39.189671
2560.949455	382637.269331	39.194688
2563.418274	383230.869694	39.199706
2565.988476	383824.491129	39.204724
2568.563951	384406.777590	39.209741
2571.103547	385003.719322	39.214759
2574.166248	385587.219432	39.219776
2576.732665	386173.999778	39.224794
2579.513510	386757.390305	39.229812
2582.258473	387345.052351	39.234829
2584.517795	387925.914370	39.239847
2587.599075	388510.837597	39.244864
2590.351545	389101.065133	39.249882
2592.927810	389688.546280	39.254900
2595.440154	390268.782108	39.259917
2598.054028	390857.444792	39.264935
2600.960405	391438.249601	39.269952
2603.185166	392027.198140	39.274970
2605.700352	392612.441358	39.279988
2608.580720	393183.993169	39.285005
2611.131133	393781.253115	39.290023
2613.521846	394360.043241	39.295040
2616.488574	394949.766378	39.300058
2618.825084	395536.586489	39.305076
2621.440056	396124.614233	39.310093
2623.988927	396719.269611	39.315111
2626.742710	397301.070159	39.320128
2629.593004	397891.852043	39.325146
2632.002251	398486.940213	39.330164
2634.763490	399074.010854	39.335181
2637.185030	399668.054589	39.340199
2640.010131	400258.426177	39.345216
2642.731394	400845.964439	39.350234
2645.053798	401432.234128	39.355252
2647.591856	401990.263395	39.360269
2649.872258	402564.464694	39.365287
2652.489906	403120.328223	39.370304
2655.004942	403691.680825	39.375322
2657.333658	404262.187833	39.380340
2660.360537	404837.075300	39.385357
2662.344422	405414.388491	39.390375
2665.310403	405985.561903	39.395392
2667.704473	406595.521722	39.400410
2669.979815	407189.037822	39.405428
2673.195401	407781.328423	39.410445
2675.380123	408376.800372	39.415463
2678.083211	408981.839391	39.420480
2680.644985	409591.336372	39.425498
2682.885102	410199.298287	39.430516
2685.994227	410810.800731	39.435533
2688.576455	411430.766723	39.440551
2691.245441	412041.999851	39.445568
2693.972862	412670.811658	39.450586
2696.639298	413308.113425	39.455604
2699.725185	413917.154136	39.460621
2702.513883	414551.111770	39.465639
2704.887227	415188.808132	39.470656
2707.484315	415816.890436	39.475674
2709.805381	416463.914352	39.480692
2713.042019	417102.227473	39.485709
2715.531806	417745.746354	39.490727
2718.266780	418387.082993	39.495744
2720.987344	419039.983700	39.500762
2723.727553	419694.428644	39.505780
2726.810188	420342.124067	39.510797
2729.679137	421000.249935	39.515815
2732.436715	421663.580708	39.520832
2735.216988	422313.688800	39.525850
2738.115694	422978.472012	39.530868
2741.268521	423633.688043	39.535885
2743.966924	424291.734920	39.540903
2746.932446	424954.976876	39.545920
2749.703498	425596.234809	39.550938
2752.526094	426258.495696	39.555956
2755.365785	426903.998502	39.560973
2758.565949	427572.678492	39.565991
2761.625165	428227.658723	39.571008
2764.576273	428878.691420	39.576026
2767.120164	429521.274360	39.581044
2770.010515	430170.858711	39.586061
2772.682489	430808.931606	39.591079
2775.692786	431467.704036	39.596096
2778.361166	432110.536707	39.601114
2781.351376	432763.709033	39.606132
2784.209245	433399.798285	39.611149
2786.933392	434051.907580	39.616167
2789.673720	434694.289698	39.621184
2792.590610	435335.763721	39.626202
2795.417946	435989.913649	39.631220
2798.109754	436625.518094	39.636237
2801.381911	437285.314475	39.641255
2803.948423	437923.623701	39.646272
2806.830524	438570.956470	39.651290
2809.729750	439212.757426	39.656308
2812.668496	439852.812631	39.661325
2815.670708	440503.950318	39.666343
2818.473068	441148.933496	39.671360
2821.640563	441780.248574	39.676378
2823.807500	442420.235568	39.681396
2826.978155	443053.224383	39.686413
2829.289092	443688.144363	39.691431
2832.425154	444319.377845	39.696448
2835.246878	444933.971488	39.701466
2837.690943	445542.290419	39.706484
2840.646454	446136.721614	39.711501
2843.603989	446741.082028	39.716519
2846.202161	447351.134597	39.721536
2848.938530	447954.681199	39.726554
2851.272244	448583.670608	39.731572
2854.055844	449196.156784	39.736589
2856.893933	449818.611287	39.741607
2859.723959	450445.135269	39.746624
2862.503536	451076.340748	39.751642
2864.935400	451717.625391	39.756660
2867.702861	452340.255455	39.761677
2870.491327	452990.374432	39.766695
2873.302802	453646.624776	39.771712
2876.149554	454298.352376	39.776730
2878.678594	454970.397979	39.781748
2881.627419	455630.742470	39.786765
2884.317955	456294.938481	39.791783
2886.985160	456980.715265	39.796800
2890.013416	457659.493971	39.801818
2892.898910	458334.937421	39.806836
2895.844124	459025.535677	39.811853
2898.606276	459710.079034	39.816871
2901.356075	460415.942842	39.821888
2904.584366	461109.087467	39.826906
2907.416238	461816.747576	39.831924
2910.270569	462513.425601	39.836941
2913.447705	463219.812698	39.841959
2916.353296	463929.593032	39.846976
2919.574638	464637.175155	39.851994
2922.259383	465346.223913	39.857012
2925.029759	466076.769717	39.862029
2928.022763	466787.424285	39.867047
2931.113846	467503.379974	39.872064
2934.408533	468225.376094	39.877082
2937.707167	468950.013237	39.882100
2940.253795	469673.727407	39.887117
2943.529609	470388.671656	39.892135
2946.580727	471108.713332	39.897152
2949.748754	471825.931412	39.902170
2952.841743	472544.037302	39.907188
2955.672331	473270.573259	39.912205
2959.452541	473979.885562	39.917223
2962.145940	474704.966669	39.922240
2965.274271	475419.661972	39.927258
2968.294080	476131.015007	39.932276
2971.380811	476843.182950	39.937293
2974.533000	477558.232658	39.942311
2977.601683	478277.195102	39.947328
2980.678468	478982.665279	39.952346
2983.629518	479686.208286	39.957364
2986.589364	480400.907635	39.962381
2989.557226	481109.222933	39.967399
2992.731085	481824.983133	39.972416
2995.928885	482524.227771	39.977434
2998.825100	483238.101953	39.982452
3001.340260	483946.661578	39.987469
3004.783091	484655.396454	39.992487
3007.835615	485372.120724	39.997504
3010.813333	486067.511316	40.002522
3013.545716	486783.061088	40.007540
3016.510662	487492.898692	40.012557
3019.872511	488204.404403	40.017575
3022.549366	488928.829263	40.022592
3025.728967	489632.539112	40.027610
3028.943712	490351.170336	40.032628
3031.516318	491050.778850	40.037645
3034.749342	491726.983310	40.042663
3037.171202	492407.816745	40.047680
3040.289091	493085.237025	40.052698
3042.714037	493757.447406	40.057716
3046.125295	494441.457780	40.062733
3048.944445	495133.938175	40.067751
3051.728130	495820.148308	40.072768
3054.805716	496512.674848	40.077786
3057.497074	497223.051639	40.082804
3060.557856	497925.935889	40.087821
3063.531528	498637.257334	40.092839
3066.239795	499346.219777	40.097856
3069.270825	500061.137609	40.102874
3072.580512	500795.556433	40.107892
3075.227541	501523.045696	40.112909
3078.322047	502252.894499	40.117927
3081.218309	503011.926293	40.122944
3084.225065	503744.632126	40.127962
3087.484782	504494.420273	40.132980
3090.665413	505242.671950	40.137997
3093.548592	505997.874383	40.143015
3096.679391	506768.695499	40.148032
3099.860404	507530.411126	40.153050
3102.780928	508305.910581	40.158068
3106.034730	509073.417524	40.163085
3109.587657	509848.280428	40.168103
3112.386167	510627.493860	40.173120
3115.517931	511400.525970	40.178138
3118.831752	512184.852995	40.183156
3121.878715	512965.254863	40.188173
3125.206740	513750.949611	40.193191
3128.244092	514546.450632	40.198208
3131.770274	515315.733154	40.203226
3134.731597	516116.686306	40.208244
3138.291888	516913.577495	40.213261
3141.184463	517704.544145	40.218279
3144.351524	518506.179752	40.223296
3147.488711	519295.557864	40.228314
3150.979976	520103.281544	40.233332
3154.109618	520902.770671	40.238349
3157.693705	521685.857686	40.243367
3160.633188	522483.573842	40.248384
3164.266203	523282.892899	40.253402
3167.496194	524076.800238	40.258420
3170.691692	524868.555327	40.263437
3173.892057	525661.116608	40.268455
3177.303057	526457.466039	40.273472
3180.602014	527248.610567	40.278490
3184.060549	528032.700097	40.283508
3187.365852	528825.306085	40.288525
3190.868078	529610.047991	40.293543
3193.574888	530387.534272	40.298560
3196.598562	531184.059249	40.303578
3199.755215	531965.900903	40.308596
3203.107560	532761.474192	40.313613
3206.451237	533552.781995	40.318631
3209.858475	534346.591988	40.323648
3213.166990	535134.594639	40.328666
3216.526937	535931.979093	40.333684
3219.204851	536716.769950	40.338701
3222.916753	537499.744548	40.343719
3225.836608	538279.783121	40.348736
3229.032956	539071.926968	40.353754
3232.265976	539856.035593	40.358772
3235.495757	540648.476885	40.363789
3239.028905	541431.487046	40.368807
3242.056407	542227.122251	40.373824
3245.462984	542996.656744	40.378842
3248.441058	543746.191998	40.383860
3251.168654	544496.925381	40.388877
3254.602509	545259.191764	40.393895
3257.223492	546007.743436	40.398912
3260.620107	546768.217156	40.403930
3263.512933	547525.312055	40.408948
3266.546582	548295.579020	40.413965
3269.969553	549061.072732	40.418983
3273.221935	549839.232615	40.424000
3275.887967	550616.481824	40.429018
3279.102459	551405.429034	40.434036
3281.846042	552207.735328	40.439053
3285.407825	553007.454116	40.444071
3288.251734	553811.894418	40.449088
3291.545912	554630.597354	40.454106
3295.123146	555438.924750	40.459124
3298.440012	556272.499378	40.464141
3300.998027	557100.471252	40.469159
3304.833736	557926.131218	40.474176
3307.910111	558767.136300	40.479194
3311.176563	559608.102150	40.484212
3314.344613	560457.290667	40.489229
3318.262155	561298.986318	40.494247
3321.437291	562159.473792	40.499264
3324.607703	563014.739386	40.504282
3328.207425	563866.369143	40.509300
3331.243119	564729.544523	40.514317
3334.492789	565593.624076	40.519335
3338.129930	566464.739844	40.524352
3341.630387	567335.410836	40.529370
3345.020287	568204.681557	40.534388
3348.171236	569087.542043	40.539405
3351.706814	569956.206973	40.544423
3355.057628	570852.717545	40.549440
3358.654755	571732.501081	40.554458
3362.328646	572605.898243	40.559476
3365.890710	573495.210703	40.564493
3369.468288	574366.685632	40.569511
3372.914115	575246.070158	40.574528
3376.107304	576132.430477	40.579546
3379.589116	577013.172312	40.584564
3383.481525	577894.030866	40.589581
3386.745567	578767.814886	40.594599
3390.352315	579653.981710	40.599616
3393.798730	580544.304251	40.604634
3397.031184	581418.134958	40.609652
3400.587554	582301.947495	40.614669
3404.050450	583181.453508	40.619687
3407.450963	584061.448934	40.624704
3410.731806	584945.142137	40.629722
3414.625455	585823.119106	40.634740
3417.984706	586712.955985	40.639757
3421.391622	587591.116520	40.644775
3424.972443	588473.976834	40.649792
3428.766827	589353.583319	40.654810
3431.835490	590234.330958	40.659828
3435.054753	591112.434712	40.664845
3438.522559	591982.583639	40.669863
3441.674520	592872.844718	40.674880
3445.280364	593756.066927	40.679898
3449.000932	594637.100081	40.684916
3452.216094	595528.378245	40.689933
3455.972335	596409.708230	40.694951
3459.279529	597287.739047	40.699968
3462.855836	598175.042294	40.704986
3466.252097	599062.298860	40.710004
3469.614794	599947.189091	40.715021
3472.996244	600802.860425	40.720026
3476.283989	601630.525748	40.725031
3479.313176	602430.092617	40.730036
3482.831604	603154.365021	40.735040
3485.406472	603846.262037	40.740045
3488.362620	604463.256445	40.745050
3491.212679	605036.855812	40.750055
3493.711509	605567.806005	40.755060
3496.441066	606038.764398	40.760064
3498.786045	606462.190758	40.765069
3500.991980	606829.549168	40.770074
3503.151120	607147.433642	40.775079
3505.181575	607417.312067	40.780084
3506.710570	607628.142947	40.785088
3508.436777	607820.683146	40.790093
3510.178574	607962.002626	40.795098
3511.541925	608066.119003	40.800103
3512.808184	608137.540668	40.805108
3513.963974	608183.822418	40.810112
3515.377718	608202.906471	40.815117
3515.877981	608175.320864	40.820122
3517.549679	608131.447689	40.825127
3518.117639	608049.636274	40.830132
3519.009361	607939.915535	40.835136
3519.689136	607826.475625	40.840141
3520.530106	607682.999833	40.845146
3520.799776	607516.203602	40.850151
3521.188457	607357.488872	40.855156
3521.652677	607161.146163	40.860160
3521.485721	606975.702531	40.865165
3521.700733	606745.427715	40.870170
3522.255413	606534.853107	40.875175
3522.425119	606306.176223	40.880180
3522.660070	606063.077249	40.885184
3523.091994	605830.096787	40.890189
3522.796592	605563.807380	40.895194
3523.153837	605306.514049	40.900199
3523.365928	605035.829326	40.905204
3523.337308	604760.472320	40.910208
3523.354686	604484.750568	40.915213
3523.325757	604196.920795	40.920218
3523.264514	603916.993456	40.925223
3523.212388	603637.157198	40.930228
3523.570109	603341.387650	40.935232
3522.912183	603051.372731	40.940237
3522.637191	602756.486040	40.945242
3523.147861	602472.477193	40.950247
3523.041563	602182.301744	40.955252
3523.260001	601877.104329	40.960256
3522.677132	601587.086885	40.965261
3522.384670	601285.254997	40.970266
3522.824957	600984.050555	40.975271
3522.022848	600697.045535	40.980276
3522.090304	600400.587219	40.985280
3521.642213	600111.558798	40.990285
3521.603990	599820.506228	40.995290
3521.401713	599545.138467	41.000295
3521.083037	599258.218646	41.005300
3521.182152	598964.768212	41.010304
3521.148586	598691.454114	41.015309
3520.430909	598407.526922	41.020314
3520.348001	598129.049695	41.025319
3520.105013	597849.588867	41.030324
3520.039050	597580.856809	41.035328
3519.873573	597306.075514	41.040333
3519.781879	597033.828950	41.045338
3519.727197	596765.224570	41.050343
3519.614948	596500.928347	41.055348
3519.116464	596230.677408	41.060352
3518.834503	595970.700565	41.065357
3518.492481	595702.564789	41.070362
3518.699137	595453.214553	41.075367
3518.167803	595196.312253	41.080372
3518.122854	594936.172857	41.085376
3517.871864	594696.290852	41.090381
3517.774342	594443.559173	41.095386
3517.431729	594206.284564	41.100391
3516.903006	593967.731646	41.105396
3517.296495	593730.431533	41.110400
3517.010087	593479.359240	41.115405
3516.040326	593251.977846	41.120410
3516.136218	593022.571838	41.125415
3515.744635	592804.707025	41.130420
3515.548781	592581.097148	41.135424
3515.574828	592361.354854	41.140429
3515.105896	592148.096951	41.145434
3515.249971	591936.642431	41.150439
3515.240945	591732.070273	41.155444
3515.000748	591512.502479	41.160448
3514.973341	591311.531874	41.165453
3514.332249	591092.669388	41.170458
3514.690222	590887.122059	41.175463
3514.392085	590695.299702	41.180468
3514.285210	590493.574783	41.185472
3513.920835	590298.098570	41.190477
3513.754806	590107.347256	41.195482
3513.736757	589914.715720	41.200487
3513.299293	589719.691348	41.205492
3513.190664	589531.075227	41.210496
3513.116818	589348.813460	41.215501
3512.934664	589169.371366	41.220506
3512.818846	588986.408596	41.225511
3512.626730	588819.037472	41.230516
3512.673772	588631.483643	41.235520
3512.185170	588457.589347	41.240525
3511.818200	588293.494397	41.245530
3511.855230	588128.582176	41.250535
3511.555345	587961.214645	41.255540
3511.511466	587801.922362	41.260544
3511.093362	587643.237464	41.265549
3510.976672	587486.457481	41.270554
3511.321273	587335.566491	41.275559
3510.726106	587186.323711	41.280564
3511.026251	587020.501613	41.285568
3510.435073	586878.119564	41.290573
3510.890207	586738.278297	41.295578
3510.482779	586587.043459	41.300583
3510.354012	586451.800214	41.305588
3509.967366	586297.400772	41.310592
3509.714119	586162.423982	41.315597
3509.707182	586032.218376	41.320602
3510.069647	585889.223257	41.325607
3509.702429	585759.672151	41.330612
3509.880669	585632.590364	41.335616
3509.424403	585497.887696	41.340621
3509.390241	585368.029275	41.345626
3509.239623	585239.841542	41.350631
3509.133856	585103.976544	41.355636
3509.165239	584977.411329	41.360640
3508.805837	584865.391492	41.365645
3509.069785	584736.180702	41.370650
3508.817883	584620.332108	41.375655
3508.701087	584503.909791	41.380660
3508.629393	584379.308668	41.385664
3508.433498	584271.868783	41.390669
3507.955635	584148.080424	41.395674
3508.368883	584039.640754	41.400679
3507.963778	583925.663486	41.405684
3508.218274	583812.734876	41.410688
3507.771897	583711.494463	41.415693
3507.961793	583607.346403	41.420698
3508.179102	583494.620857	41.425703
3508.074688	583389.213362	41.430708
3507.753927	583283.688285	41.435712
3507.724048	583184.533537	41.440717
3507.369080	583083.724234	41.445722
3507.664542	582981.358492	41.450727
3506.756133	582883.591678	41.455732
3507.002390	582781.031235	41.460736
3507.229501	582691.457439	41.465741
3506.794067	582598.878181	41.470746
3506.996832	582499.530496	41.475751
3506.787857	582415.637690	41.480756
3506.578241	582329.538396	41.485760
3506.452271	582249.792575	41.490765
3506.295702	582158.820502	41.495770
3506.391564	582069.964083	41.500775
3506.081985	581986.585106	41.505780
3506.114636	581904.605977	41.510784
3506.251781	581831.785068	41.515789
3506.094403	581750.285738	41.520794
3506.340526	581670.678119	41.525799
3506.056628	581592.656942	41.530804
3506.023384	581509.832831	41.535808
3506.083265	581436.219174	41.540813
3505.639540	581355.864765	41.545818
3505.739469	581280.689484	41.550823
3505.627598	581212.014902	41.555828
3506.027261	581132.479692	41.560832
3505.784050	581065.579658	41.565837
3505.671046	580992.190639	41.570842
3505.764962	580914.205898	41.575847
3505.487693	580847.360012	41.580852
3506.000516	580767.503642	41.585856
3505.331315	580704.428694	41.590861
3505.379864	580627.301451	41.595866
3505.443860	580554.182720	41.600871
3505.271057	580498.299769	41.605876
3505.740349	580426.972152	41.610880
3505.201917	580361.518047	41.615885
3505.052866	580282.563966	41.620890
3505.178191	580225.529856	41.625895
3505.493875	580161.244810	41.630900
3505.522365	580089.332051	41.635904
3505.080168	580026.869649	41.640909
3505.070373	579959.976601	41.645914
3505.183988	579900.184625	41.650919
3504.995143	579835.374813	41.655924
3504.936930	579763.222765	41.660928
3504.785485	579720.471025	41.665933
3504.766537	579654.430070	41.670938
3505.130098	579597.355495	41.675943
3504.983633	579539.407551	41.680948
3505.267096	579469.757727	41.685952
3504.760586	579412.015849	41.690957
3505.081999	579350.232645	41.695962
3504.871039	579277.298946	41.700967
3504.812156	579222.194153	41.705972
3504.741338	579160.421064	41.710976
3504.707276	579109.775145	41.715981
3504.279799	579054.526545	41.720986
3505.178125	578991.598015	41.725991
3504.693143	578939.667756	41.730996
3504.351884	578880.392769	41.736000
3504.655132	578823.524266	41.741005
3504.368113	578773.568328	41.746010
3504.504540	578710.907777	41.751015
3504.328463	578655.467443	41.756020
3504.467799	578604.441059	41.761024
3504.302259	578552.358752	41.766029
3504.000195	578501.952577	41.771034
3504.139857	578454.636744	41.776039
3504.302955	578420.657720	41.781044
3504.117941	578369.129284	41.786048
3504.117914	578322.837792	41.791053
3504.093273	578269.929688	41.796058
3504.549175	578225.372045	41.801063
3504.192502	578173.368004	41.806068
3503.944599	578116.732526	41.811072
3504.269909	578078.564302	41.816077
3503.884950	578026.413534	41.821082
3504.201656	577967.933625	41.826087
3504.083752	577928.780924	41.831092
3504.169942	577878.461705	41.836096
3504.069828	577835.143003	41.841101
3503.518685	577798.615504	41.846106
3504.051321	577740.200961	41.851111
3503.840220	577696.347356	41.856116
3503.822531	577649.604433	41.861120
3503.987595	577612.563111	41.866125
3504.049112	577563.600560	41.871130
3504.040711	577520.968498	41.876135
3503.922281	577482.867614	41.881140
3503.855389	577427.203489	41.886144
3504.074628	577391.758003	41.891149
3503.755532	577330.916445	41.896154
3504.088386	577288.129834	41.901159
3504.078240	577249.860755	41.906164
3503.589089	577194.060850	41.911168
3504.032313	577153.914867	41.916173
3503.683450	577117.704630	41.921178
3503.940952	577064.194973	41.926183
3503.947552	577024.718693	41.931188
3503.866784	576978.484423	41.936192
3503.450101	576943.538208	41.941197
3503.531909	576908.965394	41.946202
3503.983319	576853.317712	41.951207
3503.352076	576823.420655	41.956212
3503.219125	576776.842590	41.961216
3503.700574	576735.284649	41.966221
3503.738861	576692.642139	41.971226
3503.774415	576655.467422	41.976231
3503.602594	576621.184174	41.981236
3503.777918	576572.349988	41.986240
3503.740942	576531.022820	41.991245
3503.294291	576492.317782	41.996250
3503.657943	576451.629954	42.001255
3503.412164	576420.417518	42.006260
3503.616700	576382.964674	42.011264
3503.780072	576337.090891	42.016269
3503.570163	576291.726738	42.021274
3504.002043	576255.943452	42.026279
3503.522507	576216.690816	42.031284
3503.667405	576162.391864	42.036288
3503.570397	576127.694111	42.041293
3503.436644	576087.082724	42.046298
3503.468105	576055.474790	42.051303
3503.391711	576018.817102	42.056308
3503.341616	575983.660098	42.061312
3502.849343	575948.070469	42.066317
3503.045451	575923.108227	42.071322
3503.182966	575873.975935	42.076327
3502.918255	575850.088855	42.081332
3503.381573	575818.613402	42.086336
3503.554857	575793.052466	42.091341
3503.699220	575763.382483	42.096346
3503.502508	575720.421870	42.101351
3503.378008	575687.482830	42.106356
3503.488675	575649.289743	42.111360
3503.292537	575598.201796	42.116365
3503.090709	575561.110737	42.121370
3503.239576	575525.921200	42.126375
3503.328702	575495.907987	42.131380
3503.200090	575462.467272	42.136384
3503.363330	575431.689810	42.141389
3503.203630	575393.237123	42.146394
3503.328061	575346.713231	42.151399
3502.917453	575332.780848	42.156404
3503.183480	575297.120781	42.161408
3503.082862	575269.644970	42.166413
3503.194735	575224.677714	42.171418
3503.188328	575187.655209	42.176423
3502.948817	575154.381419	42.181428
3502.999445	575133.303067	42.186432
3502.886335	575102.016064	42.191437
3502.920770	575076.675882	42.196442
3502.733883	575041.988833	42.201447
3502.694961	575018.516203	42.206452
3502.612659	574990.183990	42.211456
3502.922823	574964.850621	42.216461
3502.866618	574942.785248	42.221466
3502.940319	574910.465142	42.226471
3502.749198	574882.500850	42.231476
3503.008380	574843.077767	42.236480
3503.446542	574815.667131	42.241485
3502.898687	574787.407188	42.246490
3503.079221	574751.708596	42.251495
3503.040571	574725.074648	42.256500
3503.235475	574686.814966	42.261504
3502.697876	574664.222269	42.266509
3502.896820	574633.587560	42.271514
3503.246023	574601.725199	42.276519
3502.813911	574567.978088	42.281524
3502.697172	574533.479191	42.286528
3502.791302	574510.034874	42.291533
3502.957388	574494.506187	42.296538
3502.834442	574455.843878	42.301543
3502.997916	574434.194705	42.306548
3502.724739	574403.683350	42.311552
3502.907440	574368.886285	42.316557
3502.903775	574344.704349	42.321562
3502.872118	574314.556365	42.326567
3502.913068	574291.019566	42.331572
3502.792407	574259.129352	42.336576
3503.062134	574232.646722	42.341581
3503.266815	574205.371452	42.346586
3503.145965	574166.005420	42.351591
3503.033037	574136.973449	42.356596
3503.095200	574098.933217	42.361600
3502.845416	574078.351411	42.366605
3503.074338	574040.987327	42.371610
3503.530249	574010.360933	42.376615
3503.307324	573979.690059	42.381620
3503.343171	573945.416377	42.386624
3503.045008	573900.307262	42.391629
3502.794628	573879.173282	42.396634
3503.243787	573835.000714	42.401639
3502.946837	573808.404988	42.406644
3503.091815	573774.013380	42.411648
3503.238264	573751.512612	42.416653
3503.141315	573723.681252	42.421658
3503.158140	573689.058551	42.426663
3503.326980	573654.060762	42.431668
3502.993761	573613.622177	42.436672
3503.064256	573590.330175	42.441677
3502.774540	573558.865811	42.446682
3502.808844	573524.189700	42.451687
3503.128819	573515.007801	42.456692
3503.196199	573475.258719	42.461696
3502.903989	573432.203979	42.466701
3502.899361	573397.734268	42.471706
3502.782001	573367.095407	42.476711
3502.835085	573354.191945	42.481716
3502.942034	573318.199286	42.486720
3502.976580	573297.872664	42.491725
3502.949155	573274.093562	42.496730
3503.202416	573235.167569	42.501735
3502.967771	573193.909260	42.506740
3502.959950	573167.567886	42.511744
3502.529267	573148.417603	42.516749
3502.324869	573121.705442	42.521754
3502.569721	573096.980228	42.526759
3502.594908	573079.665274	42.531764
3502.557736	573047.457536	42.536768
3502.685368	573026.814816	42.541773
3502.347087	572999.119758	42.546778
3502.521414	572979.322661	42.551783
3502.876677	572963.260534	42.556788
3502.857952	572928.189475	42.561792
3502.660600	572900.472144	42.566797
3502.604876	572873.083848	42.571802
3502.922498	572846.791208	42.576807
3502.626798	572828.171237	42.581812
3502.563983	572800.131562	42.586816
3502.684758	572767.898340	42.591821
3502.572076	572744.482704	42.596826
3502.748457	572717.960957	42.601831
3502.664961	572701.615804	42.606836
3502.433879	572673.301051	42.611840
3502.421812	572645.855204	42.616845
3503.007841	572628.100636	42.621850
3502.749220	572599.890363	42.626855
3502.388268	572566.929018	42.631860
3502.644619	572544.509037	42.636864
3502.427229	572514.987452	42.641869
3502.566476	572495.546252	42.646874
3502.235127	572483.655306	42.651879
3502.414040	572456.430043	42.656884
3502.311892	572429.399191	42.661888
3502.281403	572409.131326	42.666893
3501.997236	572397.985608	42.671898
3502.291890	572380.978722	42.676903
3502.333085	572367.423663	42.681908
3502.223242	572345.311435	42.686912
3502.321111	572318.750851	42.691917
3502.355614	572308.107209	42.696922
3502.386325	572271.019190	42.701927
3502.325747	572261.193251	42.706932
3502.519359	572237.728688	42.711936
3502.788713	572218.969202	42.716941
3502.747584	572192.931859	42.721946
3502.374916	572163.333274	42.726951
3502.486211	572152.677481	42.731956
3502.630331	572121.743480	42.736960
3502.576271	572100.625674	42.741965
3502.357517	572072.959851	42.746970
3502.331722	572054.647684	42.751975
3502.537307	572041.267262	42.756980
3502.308229	572006.326606	42.761984
3502.446698	571988.440286	42.766989
3502.403458	571975.349593	42.771994
3502.281943	571946.915539	42.776999
3502.370789	571939.273956	42.782004
3502.618609	571902.502069	42.787009
3502.523646	571882.042617	42.792013
3502.499529	571869.099358	42.797018
3502.457347	571840.803183	42.802023
3502.669545	571833.393157	42.807028
3503.002389	571807.196105	42.812033
3502.701658	571763.734913	42.817037
3502.349407	571750.892999	42.822042
3502.714584	571721.980839	42.827047
3502.503146	571698.879585	42.832052
3502.262692	571670.112154	42.837057
3502.617902	571658.514477	42.842061
3501.862435	571638.007293	42.847066
3502.417269	571617.194868	42.852071
3502.124412	571591.145318	42.857076
3502.407474	571581.616355	42.862081
3502.288487	571554.234775	42.867085
3501.928200	571547.867544	42.872090
3502.407470	571517.632262	42.877095
3502.562822	571483.432841	42.882100
3502.454787	571469.046919	42.887105
3502.344627	571452.804508	42.892109
3502.169421	571424.427728	42.897114
3502.072715	571399.601675	42.902119
3502.779934	571390.759006	42.907124
3502.718307	571369.942135	42.912129
3502.647934	571347.420325	42.917133
3502.399819	571328.740273	42.922138
3502.608741	571297.342246	42.927143
3502.528293	571275.775377	42.932148
3502.305073	571245.699380	42.937153
3502.501914	571237.588783	42.942157
3502.528026	571204.462611	42.947162
3502.497034	571178.220625	42.952167
3502.463357	571168.690649	42.957172
3502.797195	571150.973216	42.962177
3502.562933	571131.638268	42.967181
3502.089023	571100.346446	42.972186
3502.210357	571080.955821	42.977191
3502.605943	571058.410785	42.982196
3502.569995	571045.568812	42.987201
3502.259899	571015.606161	42.992205
3502.430002	571003.384344	42.997210
3502.645824	570973.891411	43.002215
3502.231893	570949.164156	43.007220
3502.191045	570925.181502	43.012225
3502.703772	570907.435727	43.017229
3502.618901	570896.458126	43.022234
3502.555518	570867.811549	43.027239
3502.657884	570850.581515	43.032244
3502.024817	570816.503350	43.037249
3502.498354	570789.880480	43.042253
3502.379000	570764.103038	43.047258
3502.430881	570730.921278	43.052263
3502.614915	570720.503714	43.057268
3502.326307	570706.897866	43.062273
3502.749333	570680.081889	43.067277
3502.669308	570666.393197	43.072282
3502.473171	570634.504613	43.077287
3502.512586	570608.802375	43.082292
3502.466430	570591.946483	43.087297
3502.517604	570568.902261	43.092301
3502.301633	570548.760461	43.097306
3502.249183	570531.403586	43.102311
3502.493727	570513.397999	43.107316
3502.258734	570492.907759	43.112321
3502.276015	570484.423195	43.117325
3502.486444	570461.353861	43.122330
3502.352148	570430.559181	43.127335
3502.267807	570414.160691	43.132340
3502.380809	570388.747586	43.137345
3502.287766	570360.957580	43.142349
3502.283739	570349.715872	43.147354
3502.242651	570338.429757	43.152359
3502.588077	570314.987703	43.157364
3502.334053	570277.586398	43.162369
3502.710012	570264.628967	43.167373
3501.993800	570245.016535	43.172378
3502.179241	570227.421253	43.177383
3502.482636	570202.530052	43.182388
3502.221238	570182.495087	43.187393
3502.347608	570163.503637	43.192397
3502.173494	570152.137756	43.197402
3502.509074	570120.465753	43.202407
3502.430235	570102.660645	43.207412
3502.212032	570082.618753	43.212417
3502.384749	570056.442727	43.217421
3502.103469	570043.888932	43.222426
3502.230024	570025.399125	43.227431
3502.195249	570016.320071	43.232436
3502.252073	569988.957445	43.237441
3502.101914	569971.564805	43.242445
3502.359546	569946.579822	43.247450
3502.467324	569928.996223	43.252455
3502.909378	569900.770116	43.257460
3502.224658	569887.978075	43.262465
3502.289256	569858.154576	43.267469
3502.158470	569856.117121	43.272474
3502.263043	569827.491874	43.277479
3502.276720	569815.744964	43.282484
3502.001234	569788.985912	43.287489
3502.317073	569770.616677	43.292493
3502.188151	569758.741428	43.297498
3502.645644	569724.941242	43.302503
3502.357740	569709.928735	43.307508
3502.278457	569686.903134	43.312513
3501.945973	569665.071478	43.317517
3501.749767	569647.284010	43.322522
3501.912844	569633.405504	43.327527
3501.998864	569620.944400	43.332532
3502.004559	569606.839506	43.337537
3502.311058	569593.189490	43.342541
3501.756029	569582.786047	43.347546
3501.900753	569555.007108	43.352551
3502.061635	569537.665569	43.357556
3502.135580	569524.051826	43.362561
3502.257003	569496.627735	43.367565
3502.374967	569490.084200	43.372570
3502.055703	569466.242400	43.377575
3502.442180	569457.548783	43.382580
3502.249084	569437.903378	43.387585
3502.597549	569415.362482	43.392589
3501.897033	569403.626414	43.397594
3501.897836	569383.599254	43.402599
3502.099572	569354.355323	43.407604
3502.655286	569350.102349	43.412609
3502.526751	569315.639677	43.417613
3502.101409	569323.335461	43.422618
3501.980129	569292.686267	43.427623
3502.117596	569265.459889	43.432628
3501.961867	569247.866248	43.437633
3502.062162	569231.286621	43.442637
3502.406807	569225.109048	43.447642
3502.199223	569206.519577	43.452647
3502.333759	569194.753138	43.457652
3501.953323	569178.951300	43.462657
3502.520094	569156.074607	43.467661
3502.052442	569148.919712	43.472666
3502.407424	569119.450451	43.477671
3501.937751	569112.847984	43.482676
3502.306083	569083.727904	43.487681
3502.457344	569062.070447	43.492685
3501.989752	569044.324469	43.497690
3502.289602	569016.921535	43.502695
3502.484761	569005.195620	43.507700
3502.311440	568984.391872	43.512705
3502.299258	568955.431342	43.517709
3502.213113	568938.278101	43.522714
3502.511807	568928.895081	43.527719
3502.274401	568903.633857	43.532724
3502.085404	568892.369442	43.537729
3502.493644	568858.474021	43.542733
3502.430611	568844.830692	43.547738
3502.495742	568816.560460	43.552743
3502.377449	568802.624548	43.557748
3502.196862	568770.176195	43.562753
3502.372418	568756.646050	43.567757
3502.188937	568736.094418	43.572762
3502.267446	568722.077446	43.577767
3502.577604	568702.854068	43.582772
3502.287066	568681.766921	43.587777
3502.169996	568648.806336	43.592781
3502.385238	568640.540443	43.597786
3502.366169	568606.158923	43.602791
3502.259316	568600.754348	43.607796
3502.442737	568583.709026	43.612801
3502.208575	568550.214303	43.617805
3502.345073	568537.141776	43.622810
3502.460344	568519.404260	43.627815
3502.014920	568500.951222	43.632820
3501.972440	568477.616263	43.637825
3502.329018	568466.768110	43.642829
3502.097918	568449.837589	43.647834
3502.086222	568432.119787	43.652839
3502.223523	568417.440692	43.657844
3501.761870	568402.654423	43.662849
3502.267818	568387.114504	43.667853
3501.961955	568367.886475	43.672858
3502.605012	568350.367375	43.677863
3502.415675	568329.313958	43.682868
3502.142443	568311.134881	43.687873
3502.172405	568279.907170	43.692877
3501.858782	568273.581008	43.697882
3502.148002	568252.603231	43.702887
3502.131689	568232.777535	43.707892
3502.553365	568218.254522	43.712897
3502.125738	568193.874841	43.717901
3502.418212	568195.184392	43.722906
3501.997866	568163.223592	43.727911
3502.257929	568153.444397	43.732916
3501.759777	568127.017469	43.737921
3502.361795	568109.554619	43.742925
3501.940947	568089.942513	43.747930
3501.917692	568062.186233	43.752935
3502.130327	568061.751326	43.757940
3502.250215	568057.465619	43.762945
3501.925010	568036.784298	43.767949
3501.907274	568025.040470	43.772954
3501.934596	567996.472943	43.777959
3501.630613	567989.191336	43.782964
3502.147862	567990.315175	43.787969
3502.263999	567967.355978	43.792973
3502.341255	567951.480899	43.797978
3501.962127	567921.721747	43.802983
3502.311724	567910.874165	43.807988
3502.072309	567905.339388	43.812993
3502.354168	567882.504713	43.817997
3501.970404	567878.598872	43.823002
3502.120468	567853.224569	43.828007
3502.403500	567834.154584	43.833012
3502.271220	567820.269868	43.838017
3502.331179	567777.038363	43.843021
3502.250502	567769.018908	43.848026
3502.016939	567754.396946	43.853031
3502.089701	567740.530280	43.858036
3502.012886	567722.168967	43.863041
3502.648777	567704.148010	43.868045
3502.014444	567682.209170	43.873050
3502.201463	567670.181970	43.878055
3502.242943	567642.966766	43.883060
3501.810778	567630.283313	43.888065
3502.422080	567609.956827	43.893069
3502.358346	567597.717749	43.898074
3501.899505	567577.307497	43.903079
3502.356906	567555.900558	43.908084
3501.941282	567539.800758	43.913089
3502.092152	567519.797098	43.918093
3501.878625	567504.368470	43.923098
3502.210033	567482.780288	43.928103
3502.190895	567458.134386	43.933108
3502.163879	567440.517859	43.938113
3502.567250	567434.681563	43.943117
3502.450043	567416.828092	43.948122
3502.303010	567394.059502	43.953127
3502.245481	567379.007932	43.958132
3502.223355	567353.358240	43.963137
3502.366491	567334.861522	43.968141
3501.968143	567312.132057	43.973146
3502.111681	567299.810058	43.978151
3501.746280	567292.336803	43.983156
3502.408488	567284.502089	43.988161
3502.732039	567260.304213	43.993165
3501.784157	567236.355250	43.998170
3501.887868	567219.922805	44.003175
3501.885483	567217.613794	44.008180
3501.598346	567201.945257	44.013185
3502.308957	567180.196826	44.018189
3501.644813	567182.107865	44.023194
3502.071083	567165.373905	44.028199
3501.784641	567143.078436	44.033204
3501.986984	567144.904227	44.038209
3502.243172	567112.332723	44.043213
3501.960962	567092.044607	44.048218
3501.874312	567084.628045	44.053223
3501.872675	567071.224033	44.058228
3502.015916	567043.790697	44.063233
3502.310469	567031.344399	44.068237
3501.856874	567011.785778	44.073242
3502.005030	567001.571276	44.078247
3501.948091	566981.850189	44.083252
3502.113149	566961.391516	44.088257
3502.128054	566944.570935	44.093261
3501.949623	566939.226972	44.098266
3501.768343	566924.746396	44.103271
3502.194236	566908.765179	44.108276
3501.888004	566888.530664	44.113281
3501.956359	566873.006922	44.118285
3502.027912	566877.262987	44.123290
3502.227079	566845.302092	44.128295
3502.158122	566829.548738	44.133300
3502.025142	566824.047004	44.138305
3501.600749	566799.312438	44.143309
3501.306774	566789.468093	44.148314
3501.795267	566785.274905	44.153319
3501.847419	566769.000492	44.158324
3501.708323	566758.278435	44.163329
3502.119829	566750.131125	44.168333
3501.543904	566745.752892	44.173338
3501.723042	566719.819309	44.178343
3502.278847	566710.143278	44.183348
3501.675993	566702.907577	44.188353
3502.006088	566678.707464	44.193357
3502.043545	566672.626763	44.198362
3502.338520	566656.715870	44.203367
3502.364377	566634.571418	44.208372
3502.022041	566633.319532	44.213377
3502.292352	566601.296638	44.218381
3501.946561	566582.523717	44.223386
3502.352170	566563.482684	44.228391
3502.077468	566560.463034	44.233396
3501.492923	566547.149541	44.238401
3501.709534	566521.310067	44.243405
3502.009278	566514.184172	44.248410
3502.127773	566490.870238	44.253415
3502.052315	566469.795625	44.258420
3501.858633	566473.139396	44.263425
3502.293766	566452.637605	44.268429
3502.153566	566437.145882	44.273434
3501.877076	566414.144570	44.278439
3502.074745	566404.373655	44.283444
3502.123165	566389.454852	44.288449
3501.952669	566382.201565	44.293453
3502.033253	566363.160809	44.298458
3501.891624	566346.163006	44.303463
3501.948192	566325.418933	44.308468
3502.089183	566321.681555	44.313473
3502.191798	566294.353209	44.318477
3502.032090	566285.591984	44.323482
3502.167147	566267.546683	44.328487
3502.190145	566253.736222	44.333492
3502.093348	566231.710587	44.338497
3502.084511	566210.022607	44.343501
3502.306051	566193.520080	44.348506
3502.211026	566178.422604	44.353511
3501.876546	566165.822680	44.358516
3501.861648	566155.381889	44.363521
3501.814491	566133.549136	44.368525
3502.040763	566129.396708	44.373530
3502.148868	566104.175752	44.378535
3501.900341	566091.562311	44.383540
3501.714621	566074.621209	44.388545
3502.122357	566053.068642	44.393549
3501.984522	566049.424973	44.398554
3501.938368	566043.909295	44.403559
3501.975489	566012.322889	44.408564
3501.638283	566006.049371	44.413569
3501.702193	565985.454166	44.418573
3501.929133	565979.092441	44.423578
3501.761800	565965.512223	44.428583
3501.994475	565955.534627	44.433588
3501.614007	565936.314208	44.438593
3502.020649	565924.803152	44.443597
3501.840710	565933.818428	44.448602
3502.084452	565917.412454	44.453607
3502.275148	565887.558980	44.458612
3501.863710	565887.522808	44.463617
3502.133152	565858.108822	44.468621
3501.714650	565846.023767	44.473626
3501.727077	565832.415291	44.478631
3501.656432	565814.803111	44.483636
3501.918220	565810.293558	44.488641
3501.789400	565802.581516	44.493645
3501.690311	565791.249806	44.498650
3501.779276	565771.152390	44.503655
3502.121373	565762.211904	44.508660
3501.918725	565755.565754	44.513665
3502.086944	565726.167258	44.518669
3501.996685	565724.223148	44.523674
3501.986175	565699.772990	44.528679
3501.752200	565682.487396	44.533684
3501.746701	565679.425430	44.538689
3502.049360	565662.106123	44.543693
3501.615622	565643.847518	44.548698
3501.895330	565630.548486	44.553703
3502.185361	565613.180872	44.558708
3501.718552	565598.241179	44.563713
3502.190842	565600.276064	44.568717
3502.072238	565576.495266	44.573722
3501.856111	565560.160680	44.578727
3502.064930	565556.010776	44.583732
3502.067159	565546.219485	44.588737
3502.264560	565516.916317	44.593741
3502.466437	565509.202592	44.598746
3501.712695	565480.901591	44.603751
3502.113085	565474.914155	44.608756
3501.750224	565457.999844	44.613761
3501.776507	565428.020264	44.618765
3502.131764	565427.663390	44.623770
3501.548714	565407.871242	44.628775
3502.185511	565397.629152	44.633780
3502.009477	565383.999402	44.638785
3501.764670	565359.585156	44.643789
3501.905001	565351.931158	44.648794
3501.703327	565345.083778	44.653799
3501.835192	565323.824041	44.658804
3502.109519	565309.069377	44.663809
3501.659902	565293.775129	44.668813
3501.939181	565292.676970	44.673818
3501.791532	565272.013152	44.678823
3502.080450	565262.980176	44.683828
3501.793162	565251.978626	44.688833
3501.899200	565236.999125	44.693837
3501.535747	565229.122537	44.698842
3501.650659	565218.208713	44.703847
3501.639852	565210.929727	44.708852
3501.625994	565192.303505	44.713857
3501.999780	565175.825945	44.718861
3501.729854	565172.855395	44.723866
3501.383403	565179.838624	44.728871
3501.689464	565159.204100	44.733876
3501.580230	565147.220601	44.738881
3502.097585	565142.018092	44.743885
3502.122515	565135.687488	44.748890
3501.455174	565115.205057	44.753895
3501.992246	565096.743613	44.758900
3501.765056	565096.427572	44.763905
3502.069109	565072.830729	44.768909
3502.005462	565068.271342	44.773914
3501.877630	565052.474566	44.778919
3501.927694	565023.795731	44.783924
3501.942065	565021.132181	44.788929
3501.941142	565007.173342	44.793933
3502.034540	564988.680663	44.798938
3501.597938	564973.534593	44.803943
3501.881589	564973.289326	44.808948
3501.899047	564957.469708	44.813953
3502.140153	564939.355557	44.818957
3501.985126	564936.065709	44.823962
3502.099234	564905.819993	44.828967
3501.795706	564904.612058	44.833972
3501.671958	564893.735239	44.838977
3502.036453	564874.898724	44.843981
3501.811080	564857.861620	44.848986
3501.984091	564848.545169	44.853991
3501.896527	564828.122232	44.858996
3502.077495	564814.235153	44.864001
3501.836180	564810.757908	44.869005
3501.735904	564789.583700	44.874010
3502.091786	564760.053002	44.879015
3502.324195	564758.459991	44.884020
3501.712039	564738.420184	44.889025
3501.898020	564727.595216	44.894029
3501.803816	564723.944308	44.899034
3502.047228	564705.578367	44.904039
3502.060411	564679.113831	44.909044
3501.587445	564671.253983	44.914049
3502.135826	564638.027306	44.919053
3502.288773	564633.936025	44.924058
3502.273302	564620.280279	44.929063
3502.521850	564602.114227	44.934068
3502.016647	564587.179232	44.939073
3502.486073	564567.020260	44.944077
3501.917816	564552.547002	44.949082
3501.735358	564533.443944	44.954087
3501.610662	564515.737819	44.959092
3501.953023	564516.738717	44.964097
3501.978646	564494.188510	44.969101
3501.471356	564487.790113	44.974106
3501.807683	564474.681770	44.979111
3501.840981	564463.830212	44.984116
3501.190436	564439.427248	44.989121
3501.716135	564425.385387	44.994125
3501.899639	564427.365201	44.999130
3501.517112	564430.588433	45.004135
3501.742768	564410.216227	45.009140
3501.521624	564399.555030	45.014145
3501.789582	564384.448692	45.019149
3501.894118	564389.052017	45.024154
3501.784342	564365.066505	45.029159
3502.015255	564349.011833	45.034164
3501.485225	564354.065876	45.039169
3501.713960	564340.622700	45.044173
3501.444593	564320.829872	45.049178
3501.389019	564310.594644	45.054183
3501.523989	564303.191872	45.059188
3501.996985	564306.432040	45.064193
3501.805418	564289.840753	45.069197
3501.983642	564276.204539	45.074202
3501.553391	564259.700738	45.079207
3502.120465	564259.762657	45.084212
3501.974654	564245.022114	45.089217
3502.164837	564219.683815	45.094221
3501.969196	564206.005534	45.099226
3502.148952	564189.305840	45.104231
3502.034107	564178.075453	45.109236
3501.604725	564158.960167	45.114241
3501.854669	564137.127436	45.119245
3501.687144	564143.129212	45.124250
3501.409416	564133.079204	45.129255
3501.819560	564111.070734	45.134260
3501.691810	564100.344446	45.139265
3501.513312	564093.392273	45.144269
3501.710501	564088.942374	45.149274
3501.622509	564073.740632	45.154279
3501.863850	564056.026802	45.159284
3501.483357	564055.182320	45.164289
3501.467086	564038.764136	45.169293
3501.533531	564052.362227	45.174298
3501.617497	564039.644360	45.179303
3501.512207	564019.775155	45.184308
3501.614680	564018.905385	45.189313
3501.650439	564010.111884	45.194317
3501.481552	564006.623074	45.199322
3501.577901	563992.698031	45.204327
3501.859435	563963.528457	45.209332
3501.737816	563964.099774	45.214337
3501.531353	563965.086086	45.219341
3501.477626	563954.649391	45.224346
3501.962432	563949.099931	45.229351
3501.926385	563926.859568	45.234356
3501.434895	563926.383944	45.239361
3501.717600	563907.960391	45.244365
3501.629122	563899.839046	45.249370
3501.700740	563896.111738	45.254375
3501.459755	563887.612492	45.259380
3501.241760	563885.487174	45.264385
3501.479787	563888.362459	45.269389
3501.234794	563860.831659	45.274394
3501.364572	563855.086572	45.279399
3501.636448	563846.105385	45.284404
3501.578119	563839.636443	45.289409
3501.825160	563838.442757	45.294413
3501.359883	563831.786344	45.299418
3501.706483	563814.708514	45.304423
3502.103071	563801.489563	45.309428
3501.630235	563802.969484	45.314433
3501.926425	563785.497756	45.319437
3501.909852	563769.681847	45.324442
3501.471582	563761.364002	45.329447
3501.633179	563750.441507	45.334452
3501.497599	563730.074371	45.339457
3501.415518	563724.864513	45.344461
3501.499544	563719.879774	45.349466
3501.672118	563710.562485	45.354471
3501.899842	563707.865281	45.359476
3501.596052	563696.714184	45.364481
3501.640163	563677.323216	45.369485
3501.614184	563674.213707	45.374490
3501.416014	563677.810065	45.379495
3501.500325	563673.126566	45.384500
3501.748989	563653.854235	45.389505
3501.755202	563635.222388	45.394509
3501.634465	563636.647286	45.399514
3501.427544	563626.334682	45.404519
3501.476412	563605.285661	45.409524
3501.703282	563597.315679	45.414529
3501.486690	563582.786236	45.419533
3501.520597	563575.951202	45.424538
3501.611312	563579.401992	45.429543
3501.990871	563569.700706	45.434548
3501.624447	563552.934834	45.439553
3501.494461	563544.066457	45.444557
3502.024652	563546.343753	45.449562
3501.904232	563518.340707	45.454567
3502.060914	563501.543203	45.459572
3502.247300	563506.485610	45.464577
3501.374350	563482.768246	45.469581
3501.788963	563465.779713	45.474586
3501.568121	563475.456120	45.479591
3501.863602	563454.167401	45.484596
3501.966013	563428.991766	45.489601
3501.673528	563414.423759	45.494605
3501.591011	563423.174647	45.499610
3501.413803	563407.534017	45.504615
3501.662056	563388.211094	45.509620
3501.282499	563383.750653	45.514625
3501.589622	563373.206808	45.519629
3501.779645	563375.236003	45.524634
3501.825226	563356.396682	45.529639
3501.647459	563343.618537	45.534644
3501.823404	563339.774305	45.539649
3501.587608	563340.966130	45.544653
3501.642948	563315.697172	45.549658
3501.471221	563308.291498	45.554663
3501.874296	563303.909555	45.559668
3501.427357	563300.715097	45.564673
3501.541937	563285.229565	45.569677
3501.420108	563271.387991	45.574682
3501.708043	563261.700776	45.579687
3502.138998	563255.657215	45.584692
3501.773387	563252.098493	45.589697
3502.055735	563229.154176	45.594701
3501.731049	563222.274555	45.599706
3501.800071	563215.885797	45.604711
3501.790671	563198.812505	45.609716
3502.093616	563188.771345	45.614721
3501.904016	563173.483877	45.619725
3502.015774	563141.827806	45.624730
3502.074074	563142.923455	45.629735
3502.355615	563125.955234	45.634740
3501.923190	563114.673030	45.639745
3502.018739	563104.965540	45.644749
3502.164749	563088.570873	45.649754
3501.677980	563064.691846	45.654759
3501.845557	563065.368657	45.659764
3501.830118	563049.903140	45.664769
3502.096238	563033.238517	45.669773
3501.727388	563022.197387	45.674778
3501.875721	562997.666512	45.679783
3501.660897	562980.474353	45.684788
3501.379242	562977.404628	45.689793
3501.508195	562961.966643	45.694797
3501.816730	562967.794157	45.699802
3501.502234	562942.280885	45.704807
3501.657365	562933.819460	45.709812
3501.659836	562936.631364	45.714817
3501.972000	562917.749663	45.719821
3501.706706	562899.410194	45.724826
3501.541715	562876.786225	45.729831
3501.873423	562817.071495	45.734836
3501.182408	562708.700852	45.739841
3501.157709	562565.169846	45.744845
3500.856485	562362.165868	45.749850
3500.307100	562123.236624	45.754855
3500.589293	561830.983772	45.759860
3499.877532	561497.994352	45.764865
3499.400100	561113.424423	45.769869
3498.928137	560681.272936	45.774874
3497.928868	560207.846797	45.779879
3496.937877	559682.106175	45.784884
3496.652247	559140.809174	45.789889
3495.386122	558534.530441	45.794893
3494.649988	557895.229260	45.799898
3493.367976	557219.551423	45.804903
3492.518296	556493.268409	45.809908
3491.539021	555738.268055	45.814913
3490.083637	554926.908884	45.819917
3488.654891	554082.370602	45.824922
3487.201944	553213.852268	45.829927
3485.860762	552299.813936	45.834932
3483.849030	551347.556364	45.839937
3482.960658	550369.006834	45.844941
3481.218025	549351.496791	45.849946
3479.387095	548293.388549	45.854951
3477.141889	547198.444089	45.859956
3475.410899	546087.128171	45.864961
3473.839589	544937.412336	45.869965
3471.767736	543759.399360	45.874970
3469.582081	542544.720763	45.879975
3467.531055	541306.861020	45.884980
3465.265249	540040.635600	45.889985
3463.348383	538753.546783	45.894989
3461.063630	537424.161387	45.899994
3458.570056	536074.587652	45.904999
3456.057131	534696.635678	45.910004
3453.693325	533313.629419	45.915009
3451.550004	531897.966384	45.920013
3448.889173	530461.937472	45.925018
3446.131667	529001.291147	45.930023
3443.646766	527512.789304	45.935028
3440.680776	526020.114458	45.940033
3437.886445	524497.371575	45.945037
3435.057664	522965.139242	45.950042
3432.184883	521413.742253	45.955047
3429.320354	519847.702200	45.960052
3426.083323	518267.124944	45.965057
3423.447641	516677.096331	45.970061
3420.431223	515062.846048	45.975066
3417.341271	513449.275030	45.980071
3414.756970	511801.300639	45.985076
3411.474263	510153.139611	45.990081
3408.098142	508488.761061	45.995085
3405.076779	506816.160919	46.000090
3401.414697	505133.626637	46.005095
3398.837030	503429.383003	46.010100
3395.207462	501730.097096	46.015105
3391.777692	500025.533773	46.020109
3388.604794	498301.804177	46.025114
3384.841175	496576.399334	46.030119
3381.993980	494833.737703	46.035124
3378.320030	493094.131053	46.040129
3374.650905	491356.391414	46.045133
3371.441753	489591.715147	46.050138
3367.674702	487830.455998	46.055143
3364.316135	486064.131043	46.060148
3360.685661	484308.203707	46.065153
3357.008847	482533.542308	46.070157
3353.583405	480758.487918	46.075162
3350.118658	478983.744282	46.080167
3346.548077	477203.763933	46.085172
3342.939183	475425.612468	46.090177
3339.375547	473639.067483	46.095181
3335.566623	471854.233983	46.100186
3331.806700	470074.455695	46.105191
3328.199451	468276.306489	46.110196
3324.656149	466491.657153	46.115201
3321.141913	464701.349541	46.120205
3317.401511	462909.419406	46.125210
3313.495582	461118.387723	46.130215
3310.335442	459315.970973	46.135220
3306.047847	457528.620367	46.140225
3302.087910	455732.026300	46.145229
3298.593503	453933.656260	46.150234
3294.677143	452152.276614	46.155239
3291.268314	450342.594788	46.160244
3287.137286	448553.447628	46.165249
3283.601074	446770.561397	46.170253
3279.704573	444973.783758	46.175258
3275.716261	443192.644395	46.180263
3272.177679	441411.567049	46.185268
3268.419552	439638.407381	46.190273
3264.848900	437845.143721	46.195277
3261.309784	436058.696722	46.200282
3256.934965	434272.568280	46.205287
3253.829547	432498.287415	46.210292
3249.834626	430725.656229	46.215297
3245.688872	428949.949321	46.220301
3242.203684	427168.100807	46.225306
3238.099812	425396.175735	46.230311
3234.547763	423622.082503	46.235316
3230.444924	421864.194379	46.240321
3226.574868	420109.668535	46.245325
3222.994018	418336.238932	46.250330
3218.748967	416583.756566	46.255335
3215.426679	414831.085996	46.260340
3211.199925	413079.021454	46.265345
3207.123544	411338.304633	46.270349
3203.831700	409597.579379	46.275354
3199.675645	407862.431460	46.280359
3196.409524	406126.348987	46.285364
3192.239799	404386.721495	46.290369
3188.557555	402652.262441	46.295373
3184.649149	400929.581312	46.300378
3180.882047	399201.471452	46.305383
3177.048995	397470.452245	46.310388
3173.333809	395747.763537	46.315393
3169.545878	394037.499053	46.320397
3166.035660	392319.810107	46.325402
3162.116707	390610.693877	46.330407
3158.289159	388898.372557	46.335412
3154.102320	387181.140121	46.340417
3150.286198	385474.242923	46.345421
3146.640286	383776.319200	46.350426
3142.432327	382095.002570	46.355431
3138.996199	380402.841323	46.360436
3135.515633	378720.481759	46.365441
3131.528668	377035.783198	46.370445
3127.439209	375354.270931	46.375450
3123.940878	373684.474365	46.380455
3120.350448	371999.654008	46.385460
3116.298763	370331.137497	46.390465
3112.456973	368664.444856	46.395469
3108.708702	366991.135477	46.400474
3104.804082	365338.180666	46.405479
3101.124391	363670.003388	46.410484
3097.308119	362018.345788	46.415489
3093.274304	360366.681196	46.420493
3089.901931	358725.165717	46.425498
3086.051481	357082.365757	46.430503
3082.716026	355432.637041	46.435508
3078.738234	353800.281721	46.440513
3074.709373	352163.198492	46.445517
3071.304155	350522.070234	46.450522
3067.420721	348902.668997	46.455527
3063.264332	347272.299001	46.460532
3059.539383	345642.722461	46.465537
3055.868799	344030.805462	46.470541
3052.142224	342414.422617	46.475546
3048.286791	340802.663306	46.480551
3044.526388	339189.035354	46.485556
3041.105000	337589.471217	46.490561
3037.241045	335995.322401	46.495565
3033.498629	334387.174198	46.500570
3029.419109	332790.276151	46.505575
3025.591437	331191.160317	46.510580
3022.143331	329603.262605	46.515585
3018.495724	328011.617790	46.520589
3014.882810	326442.135613	46.525594
3010.720935	324855.176671	46.530599
3007.619886	323276.079846	46.535604
3003.540128	321691.479244	46.540609
2999.568450	320124.127556	46.545613
2996.181492	318563.929013	46.550618
2992.050985	316990.942379	46.555623
2988.534659	315423.579677	46.560628
2984.595597	313863.989280	46.565633
2981.296407	312308.164495	46.570637
2977.654512	310747.099654	46.575642
2973.598930	309198.390179	46.580647
2970.146458	307642.513360	46.585652
2966.190901	306100.332179	46.590657
2962.240331	304553.598477	46.595661
2958.525010	303014.161970	46.600666
2954.687932	301490.504284	46.605671
2951.101951	299950.245796	46.610676
2947.880957	298429.154155	46.615681
2944.276005	296898.459775	46.620685
2940.694902	295361.993391	46.625690
2936.505434	293839.454157	46.630695
2932.973206	292303.892894	46.635700
2929.177363	290795.597047	46.640705
2925.541808	289280.900941	46.645709
2922.162294	287766.586974	46.650714
2918.393325	286245.959841	46.655719
2914.352190	284733.232643	46.660724
2910.476038	283232.539054	46.665729
2907.166671	281715.150925	46.670733
2903.813912	280215.992228	46.675738
2899.679365	278717.791125	46.680743
2895.983467	277215.621962	46.685748
2892.370879	275717.459311	46.690753
2888.190585	274224.399035	46.695757
2884.789448	272722.838579	46.700762
2881.361934	271240.276427	46.705767
2877.592213	269757.080952	46.710772
2874.092011	268269.796103	46.715777
2870.514524	266795.511914	46.720781
2866.991303	265310.247541	46.725786
2863.236334	263822.604066	46.730791
2859.502366	262342.703099	46.735796
2855.648747	260868.403218	46.740801
2851.708402	259395.600349	46.745805
2848.436694	257929.830588	46.750810
2844.680431	256470.027476	46.755815
2840.956053	254997.062435	46.760820
2837.466679	253540.241510	46.765825
2834.006668	252075.277331	46.770829
2830.036354	250607.883041	46.775834
2826.441250	249162.216625	46.780839
2822.815909	247702.433670	46.785844
2819.134818	246256.094595	46.790849
2815.522474	244797.611257	46.795853
2811.971090	243354.720051	46.800858
2808.064609	241909.430151	46.805863
2804.777224	240456.063266	46.810868
2800.865706	239018.601986	46.815873
2796.896645	237570.394945	46.820877
2793.742042	236129.210842	46.825882
2789.666439	234709.329743	46.830887
2786.686022	233260.772989	46.835892
2782.978741	231827.708968	46.840897
2779.107704	230395.558606	46.845901
2775.491361	228965.225007	46.850906
2771.797669	227538.543658	46.855911
2768.132613	226100.828528	46.860916
2764.414239	224687.367790	46.865921
2760.753945	223270.026889	46.870925
2757.606762	221841.604031	46.875930
2753.855358	220432.149836	46.880935
2750.020451	219007.404147	46.885940
2746.856084	217592.081987	46.890945
2742.440704	216180.804970	46.895949
2738.851395	214752.873911	46.900954
2735.111911	213343.079709	46.905959
2731.889594	211936.546728	46.910964
2728.123353	210543.246893	46.915969
2724.264252	209133.414137	46.920973
2720.932448	207726.511926	46.925978
2717.409519	206337.119054	46.930983
2713.682380	204935.822601	46.935988
2710.043397	203542.569824	46.940993
2706.104003	202140.460689	46.945997
2702.865818	200742.582364	46.951002
2698.898125	199360.950401	46.956007
2695.523906	197962.684254	46.961012
2692.150631	196583.530845	46.966017
2688.501903	195197.761638	46.971021
2684.839419	193804.063252	46.976026
2680.790271	192426.432709	46.981031
2677.102227	191041.656016	46.986036
2673.750949	189669.702543	46.991041
2670.051247	188287.735823	46.996045
2666.665490	186914.700725	47.001050
2662.742608	185556.460100	47.006055
2659.183242	184175.746842	47.011060
2655.535495	182810.420993	47.016065
2651.855674	181436.462008	47.021069
2648.482458	180070.419628	47.026074
2644.301611	178717.509947	47.031079
2640.755725	177361.058921	47.036084
2637.135180	175994.303700	47.041089
2633.703692	174650.800110	47.046093
2630.215199	173288.601398	47.051098
2626.443760	171948.862780	47.056103
2623.168456	170591.311718	47.061108
2619.619045	169251.573291	47.066113
2615.885261	167902.162972	47.071117
2612.394193	166542.455021	47.076122
2608.769417	165203.733605	47.081127
2605.263975	163853.996780	47.086132
2601.538300	162513.371648	47.091137
2597.899122	161169.234846	47.096141
2594.363527	159826.472027	47.101146
2590.548121	158487.854647	47.106151
2587.066388	157145.357942	47.111156
2583.404164	155812.401130	47.116161
2579.423477	154483.673222	47.121165
2576.349242	153147.923618	47.126170
2572.357989	151817.248482	47.131175
2568.743303	150486.266281	47.136180
2565.034982	149161.299403	47.141185
2561.412215	147847.689998	47.146189
2557.679056	146517.193687	47.151194
2554.235487	145186.660731	47.156199
2551.005754	143804.455890	47.161204
2547.490291	142501.705413	47.166209
2543.856491	141180.609556	47.171213
2540.272142	139857.124468	47.176218
2536.713935	138537.068905	47.181223
2532.833189	137223.907316	47.186228
2529.200367	135918.466445	47.191233
2525.770481	134613.056550	47.196237
2522.086919	133300.511123	47.201242
2518.438824	131995.746040	47.206247
2514.677564	130685.338697	47.211252
2510.912670	129395.832904	47.216257
2507.781531	128103.366893	47.221261
2504.256510	126796.972672	47.226266
2500.569683	125511.071745	47.231271
2496.656473	124201.284681	47.236276
2493.300330	122916.444316	47.241281
2489.531484	121630.234637	47.246285
2486.023373	120325.560496	47.251290
2482.125295	119053.915422	47.256295
2478.814418	117750.759805	47.261300
2475.099263	116472.394183	47.266305
2471.491939	115197.183341	47.271309
2467.947861	113913.207531	47.276314
2464.446771	112632.346990	47.281319
2460.708849	111356.387548	47.286324
2457.027182	110093.458398	47.291329
2453.397942	108809.563489	47.296333
2450.085266	107542.917657	47.301338
2446.115032	106275.963365	47.306343
2442.742346	105007.335321	47.311348
2439.042972	103740.763448	47.316353
2435.045310	102479.777262	47.321357
2432.086854	101225.883340	47.326362
2428.227785	99971.707885	47.331367
2424.350440	98706.132304	47.336372
2421.086967	97457.693184	47.341377
2417.559559	96198.630889	47.346381
2413.680885	94940.143980	47.351386
2410.195904	93701.076087	47.356391
2406.352467	92451.401801	47.361396
2402.855112	91215.294936	47.366401
2398.956792	89973.405501	47.371405
2395.550205	88726.509842	47.376410
2391.481987	87493.491227	47.381415
2387.804949	86257.083507	47.386420
2384.432836	85039.723489	47.391425
2380.609643	83822.358074	47.396429
2377.156625	82595.421031	47.401434
2373.078302	81380.079378	47.406439
2369.483864	80149.726216	47.411444
2366.164324	78958.516456	47.416449
2362.392599	77745.316642	47.421453
2359.255035	76526.889386	47.426458
2355.346428	75335.902939	47.431463
2351.653356	74128.921694	47.436468
2348.128440	72931.314331	47.441473
2344.201487	71735.080704	47.446477
2340.842418	70539.040856	47.451482
2337.023702	69354.275062	47.456487
2333.509838	68153.861164	47.461492
2330.060774	66974.853041	47.466497
2326.258247	65794.640457	47.471501
2322.661149	64612.933459	47.476506
2318.658907	63432.861987	47.481511
2315.225270	62260.493537	47.486516
2311.568471	61087.732863	47.491521
2307.822408	59929.834236	47.496525
2304.359476	58763.220632	47.501530
2300.612487	57598.845688	47.506535
2296.920240	56444.346698	47.511540
2293.656917	55275.979118	47.516545
2289.996861	54131.097386	47.521549
2286.655477	52973.964220	47.526554
2282.835975	51821.974347	47.531559
2279.066783	50668.783689	47.536564
2275.725558	49522.199292	47.541569
2271.923642	48378.027385	47.546573
2268.364597	47230.589156	47.551578
2264.825137	46095.706254	47.556583
2261.096125	44959.203962	47.561588
2257.311427	43824.188372	47.566593
2253.580142	42691.714237	47.571597
2249.889133	41565.518419	47.576602
2246.416580	40443.226409	47.581607
2242.248692	39327.459989	47.586612
2238.741474	38215.039265	47.591617
2235.171353	37104.669856	47.596621
2231.643225	35991.492132	47.601626
2227.564596	34894.217237	47.606631
2223.837264	33795.511471	47.611636
2220.166288	32701.233797	47.616641
2216.609800	31625.508558	47.621645
2213.348289	30535.279219	47.626650
2209.145213	29453.024001	47.631655
2205.364040	28374.048399	47.636660
2201.598970	27304.194770	47.641665
2197.593911	26246.239375	47.646669
2194.067068	25177.195193	47.651674
2190.275763	24119.184369	47.656679
2186.431590	23073.958947	47.661684
2182.557036	22035.102635	47.666689
2178.420264	21012.381125	47.671693
2174.827623	19981.348312	47.676698
2171.007398	18958.246678	47.681703
2166.559893	17949.503199	47.686708
2162.818189	16948.168614	47.691713
2158.727993	15965.793854	47.696717
2155.254448	14980.222092	47.701722
2150.991261	14020.705138	47.706727
2147.023735	13066.385620	47.711732
2142.538518	12134.758392	47.716737
2137.256461	11231.217304	47.721741
2131.881346	10353.024135	47.726746
2126.464381	9512.515982	47.731751
2121.493439	8684.804916	47.736756
2116.271852	7887.141039	47.741761
2111.135861	7135.068597	47.746765
2106.460804	6392.275384	47.751770
2101.031919	5697.915610	47.756775
2095.369714	5034.113660	47.761780
2089.860939	4404.502025	47.766785
2083.920236	3848.142703	47.771789
2078.008723	3317.316743	47.776794
2071.766735	2841.769010	47.781799
2066.096690	2398.840390	47.786804
2060.896486	1981.836437	47.791809
2055.938038	1622.226424	47.796813
2051.247529	1277.560271	47.801818
2046.448424	971.553193	47.806823
2041.730884	693.520471	47.811828
2038.031571	441.599415	47.816833
2032.882095	215.906224	47.821837
2025.192192	112.455611	47.826842
2013.946477	138.102184	47.831847
2007.077879	134.810757	47.836852
2003.505118	146.016059	47.841857
2001.366994	147.574952	47.846861
2000.248252	135.167323	47.851866
1998.488298	143.355407	47.856871
1996.238613	153.505778	47.861876
1993.899100	149.935953	47.866881
1991.374671	148.442071	47.871885
1988.827099	146.129212	47.876890
1985.377471	149.674571	47.881895
1982.076032	148.159902	47.886900
1979.132954	137.474126	47.891905
1975.506576	147.393814	47.896909
1972.149072	138.902155	47.901914
1969.044863	147.889064	47.906919
1965.961212	143.540319	47.911924
1962.708791	131.131207	47.916929
1959.089785	138.990080	47.921933
1956.100593	138.109951	47.926938
1953.039067	143.973798	47.931943
1949.575463	139.007453	47.936948
1946.648393	130.964160	47.941953
1943.023356	136.729519	47.946957
1939.497607	127.900363	47.951962
1935.586778	135.330330	47.956967
1932.308937	147.451308	47.961972
1929.381618	132.602635	47.966977
1925.890287	142.346172	47.971981
1922.597481	140.580229	47.976986
1918.800000	133.467272	47.981991
1915.394102	147.883094	47.986996
1912.468015	147.913780	47.992001
1908.996782	142.679716	47.997005
1905.335636	138.918084	48.002010
1902.054824	135.868916	48.007015
1898.869400	147.162332	48.012020
1895.951269	132.176189	48.017025
1891.960733	131.965315	48.022029
1888.047790	132.852808	48.027034
1884.644579	127.326532	48.032039
1881.154904	132.222816	48.037044
1878.355983	136.637676	48.042049
1874.542943	138.465020	48.047053
1871.779420	130.212659	48.052058
1867.511645	138.340764	48.057063
1864.067199	134.652809	48.062068
1861.386871	126.779749	48.067073
1857.619022	137.439791	48.072077
1854.252843	136.245352	48.077082
1850.376571	135.257291	48.082087
1846.424248	140.792314	48.087092
1843.479895	131.720350	48.092097
1840.318701	134.821969	48.097101
1837.326012	127.035764	48.102106
1833.191078	132.485467	48.107111
1829.348570	134.798341	48.112116
1825.773764	137.990001	48.117121
1822.730386	147.255331	48.122125
1818.927904	138.646700	48.127130
1815.638587	132.409744	48.132135
1812.299805	141.332149	48.137140
1809.477825	134.047598	48.142145
1805.598606	141.915597	48.147149
1802.166217	134.748719	48.152154
1798.493695	127.657391	48.157159
1795.156448	131.897079	48.162164
1791.776881	136.152883	48.167169
1788.310833	139.697704	48.172173
1784.812241	135.388647	48.177178
1781.206418	129.951065	48.182183
1777.368908	139.748812	48.187188
1774.237492	131.984338	48.192193
1770.357831	129.079554	48.197197
1766.966332	128.180180	48.202202
1763.587716	131.448726	48.207207
1760.190794	134.267709	48.212212
1757.191713	129.469194	48.217217
1753.516204	128.212464	48.222221
1749.993650	121.999381	48.227226
1746.540603	121.679137	48.232231
1742.822632	129.224515	48.237236
1739.249089	124.218509	48.242241
1735.507731	127.369820	48.247245
1731.859151	129.639723	48.252250
1728.944608	125.995443	48.257255
1725.383320	124.182996	48.262260
1722.144429	114.698424	48.267265
1718.572378	124.274298	48.272269
1715.120759	121.713847	48.277274
1711.695787	118.693635	48.282279
1707.675629	122.129039	48.287284
1704.425571	126.889794	48.292289
1700.671321	132.450813	48.297293
1697.896284	129.812954	48.302298
1694.274998	130.667528	48.307303
1690.409810	123.413405	48.312308
1687.151391	122.970970	48.317313
1683.136184	114.000225	48.322317
1679.842443	122.210070	48.327322
1676.522011	129.468619	48.332327
1673.495921	122.782389	48.337332
1670.181828	116.701233	48.342337
1666.332423	125.874429	48.347341
1662.756402	121.118784	48.352346
1659.226637	119.453292	48.357351
1655.385440	121.690089	48.362356
1652.073798	116.038838	48.367361
1648.346710	127.493001	48.372365
1644.994228	125.125871	48.377370
1641.554252	116.419466	48.382375
1637.616691	115.921982	48.387380
1634.863498	106.709455	48.392385
1631.299644	122.769916	48.397389
1628.134239	116.127655	48.402394
1624.393268	114.311730	48.407399
1620.695534	129.390218	48.412404
1617.113434	131.029644	48.417409
1613.695035	122.860885	48.422413
1610.251526	118.809039	48.427418
1606.761312	127.514737	48.432423
1602.943995	111.150828	48.437428
1599.827459	119.937248	48.442433
1595.778268	115.818849	48.447437
1592.620556	108.700826	48.452442
1589.570905	116.182773	48.457447
1585.689846	111.769140	48.462452
1582.304790	116.987663	48.467457
1578.463672	123.223554	48.472461
1574.966684	113.298535	48.477466
1571.854224	111.754428	48.482471
1568.355562	121.378965	48.487476
1565.026113	108.365146	48.492481
1560.994271	120.145442	48.497485
1557.973971	113.040725	48.502490
1554.413158	121.352515	48.507495
1550.629548	123.289263	48.512500
1547.307977	115.386961	48.517505
1543.579923	118.735574	48.522509
1540.131967	116.854836	48.527514
1536.658102	119.413840	48.532519
1533.611449	116.078210	48.537524
1530.375586	120.374871	48.542529
1526.310663	121.526736	48.547533
1522.729675	114.724929	48.552538
1519.237057	119.542682	48.557543
1515.454853	123.845766	48.562548
1512.729073	115.315537	48.567553
1509.038198	115.927961	48.572557
1505.657993	110.942410	48.577562
1501.710091	108.690676	48.582567
1497.951393	116.270971	48.587572
1494.890593	111.728987	48.592577
1490.990318	122.125104	48.597581
1487.836012	111.415643	48.602586
1484.165050	106.766684	48.607591
1480.897247	113.048910	48.612596
1477.432577	106.557957	48.617601
1473.643827	121.606426	48.622605
1470.138217	107.462262	48.627610
1466.603289	111.502024	48.632615
1463.242077	120.428016	48.637620
1460.000766	113.667982	48.642625
1456.483445	116.939346	48.647629
1453.460584	115.874808	48.652634
1449.098058	117.965485	48.657639
1445.713669	123.756598	48.662644
1442.554650	111.352082	48.667649
1438.987773	104.285508	48.672653
1435.785150	113.702384	48.677658
1432.046408	99.752928	48.682663
1427.832611	116.867471	48.687668
1424.817571	114.817769	48.692673
1421.243201	108.252257	48.697677
1417.592007	110.038609	48.702682
1414.170314	113.374113	48.707687
1410.840226	111.826157	48.712692
1407.351515	101.852465	48.717697
1403.670892	103.447271	48.722701
1400.538822	109.211551	48.727706
1396.917101	115.353044	48.732711
1393.167042	113.380440	48.737716
1389.618684	104.222865	48.742721
1386.297743	113.224830	48.747725
1383.153067	105.038638	48.752730
1379.128778	105.399573	48.757735
1375.654781	108.499662	48.762740
1372.644495	103.658744	48.767745
1368.746852	106.970685	48.772749
1365.397481	103.622387	48.777754
1361.829731	102.291989	48.782759
1358.261787	104.492445	48.787764
1354.709311	98.746131	48.792769
1351.478992	107.955383	48.797773
1347.911679	103.217488	48.802778
1344.675775	108.713293	48.807783
1340.513617	107.675270	48.812788
1337.213412	103.544150	48.817793
1333.573002	106.176746	48.822797
1330.168563	104.994805	48.827802
1326.784175	93.153989	48.832807
1323.219148	102.393494	48.837812
1319.723763	98.416324	48.842817
1316.611957	106.768620	48.847821
1313.265127	108.678210	48.852826
1309.251544	105.911644	48.857831
1305.531681	112.324796	48.862836
1302.387643	104.496048	48.867841
1298.745934	109.245454	48.872845
1295.527263	107.281456	48.877850
1292.026580	109.677054	48.882855
1288.258650	113.667924	48.887860
1284.545514	102.650556	48.892865
1280.949907	109.411266	48.897869
1277.157148	118.192886	48.902874
1274.241707	111.995693	48.907879
1270.990201	116.971933	48.912884
1267.596496	112.368245	48.917889
1264.223504	108.280183	48.922893
1260.674803	110.771896	48.927898
1257.080135	109.600777	48.932903
1252.876773	110.907303	48.937908
1250.097343	101.139027	48.942913
1245.975637	108.864812	48.947917
1242.344690	110.926472	48.952922
1239.290320	107.228311	48.957927
1235.313174	105.215389	48.962932
1232.170007	102.992816	48.967937
1228.801983	112.565350	48.972941
1225.227705	107.524867	48.977946
1221.991145	107.455657	48.982951
1218.087737	109.098062	48.987956
1215.036324	108.408236	48.992961
1211.471568	100.329007	48.997965
1207.684483	109.407154	49.002970
1204.038624	100.419955	49.007975
1200.486490	114.469644	49.012980
1197.285125	111.613937	49.017985
1193.729579	112.895003	49.022989
1190.327841	107.549107	49.027994
1186.724437	106.518590	49.032999
1182.873876	112.442869	49.038004
1179.936788	106.565482	49.043009
1176.396566	103.671083	49.048013
1172.781125	103.503014	49.053018
1169.359769	97.154108	49.058023
1165.913773	107.877836	49.063028
1162.348919	103.879964	49.068033
1158.631784	117.977644	49.073037
1155.050760	105.636160	49.078042
1151.654216	99.824388	49.083047
1147.966577	106.172432	49.088052
1144.675296	101.663493	49.093057
1141.044163	111.176000	49.098061
1137.519080	111.683509	49.103066
1134.430682	106.810609	49.108071
1130.849055	109.032269	49.113076
1127.355020	104.248189	49.118081
1123.723498	112.574332	49.123085
1120.317808	116.198496	49.128090
1116.533218	106.030803	49.133095
1112.856858	107.046068	49.138100
1109.829675	108.896188	49.143105
1106.403271	106.161170	49.148109
1102.983281	102.346290	49.153114
1098.975939	101.891586	49.158119
1095.387704	103.506841	49.163124
1092.437247	106.667427	49.168129
1088.415047	116.529085	49.173133
1085.094293	110.012595	49.178138
1081.865858	120.582065	49.183143
1078.330702	101.946940	49.188148
1074.770874	109.948655	49.193153
1070.970778	116.997718	49.198157
1067.585345	110.320516	49.203162
1064.037053	108.984019	49.208167
1060.786152	111.745556	49.213172
1057.409204	103.947042	49.218177
1053.569448	108.268785	49.223181
1050.301454	96.881276	49.228186
1046.752044	96.237836	49.233191
1042.827312	102.505973	49.238196
1039.753017	89.990304	49.243201
1035.874706	94.137750	49.248205
1032.402423	96.952938	49.253210
1029.265871	100.307196	49.258215
1025.755647	106.016887	49.263220
1022.245734	99.169369	49.268225
1018.991248	103.130563	49.273229
1015.135774	112.792130	49.278234
1012.004159	99.057882	49.283239
1007.855349	99.213835	49.288244
1004.165238	94.666155	49.293249
1001.118107	104.799118	49.298253
997.412730	99.165479	49.303258
994.255928	101.048583	49.308263
990.442739	110.627604	49.313268
987.502602	103.115074	49.318273
983.739795	104.764030	49.323277
979.777168	109.623903	49.328282
976.869110	100.268182	49.333287
972.810607	106.408591	49.338292
969.319103	105.930123	49.343297
965.545232	104.986495	49.348301
962.331856	101.759426	49.353306
959.335615	97.922547	49.358311
955.860620	97.615509	49.363316
952.509944	94.191640	49.368321
948.648555	103.167603	49.373325
945.228373	95.208228	49.378330
941.475035	107.489274	49.383335
937.944760	103.419639	49.388340
934.637926	95.996187	49.393345
930.797903	105.547788	49.398349
927.352478	103.053103	49.403354
924.024289	105.114928	49.408359
920.551911	104.674613	49.413364
917.302180	98.552042	49.418369
913.387526	94.460347	49.423373
909.973151	99.335639	49.428378
906.795287	100.905688	49.433383
903.230975	100.280455	49.438388
899.261623	102.407881	49.443393
895.878981	97.239454	49.448397
892.454151	103.824845	49.453402
889.341530	99.417745	49.458407
885.318013	106.704335	49.463412
882.165370	98.639817	49.468417
878.516858	105.475377	49.473421
875.030679	109.688036	49.478426
871.489592	100.757350	49.483431
868.004261	105.672243	49.488436
864.610327	98.328897	49.493441
861.069266	102.195807	49.498445
857.647941	98.662812	49.503450
854.366697	95.648894	49.508455
850.107786	106.098194	49.513460
846.773256	100.609035	49.518465
843.071740	100.720330	49.523469
840.134159	90.711219	49.528474
836.572331	96.106341	49.533479
832.914316	99.520166	49.538484
829.388691	90.422567	49.543489
825.850917	95.851891	49.548493
822.141882	96.717356	49.553498
819.085346	91.187844	49.558503
815.450771	90.526191	49.563508
812.366551	90.233946	49.568513
808.539068	91.880441	49.573517
805.097095	93.159681	49.578522
801.798811	91.973966	49.583527
797.872444	106.810026	49.588532
794.494546	99.470527	49.593537
790.989724	88.199320	49.598541
787.393799	98.373974	49.603546
783.987629	92.873915	49.608551
780.250022	101.042763	49.613556
776.878593	92.977750	49.618561
773.181303	92.828979	49.623565
770.005114	96.483755	49.628570
766.583446	92.897066	49.633575
763.031449	99.110098	49.638580
759.876085	91.764243	49.643585
756.037807	100.891676	49.648589
752.210792	100.544925	49.653594
748.731126	95.723951	49.658599
744.965709	98.692712	49.663604
742.262152	90.814197	49.668609
738.415745	96.453236	49.673613
734.892032	89.038523	49.678618
731.931427	85.060104	49.683623
727.896690	94.699207	49.688628
724.057490	89.491616	49.693633
720.394870	92.494909	49.698637
717.301417	92.333857	49.703642
714.345954	95.368781	49.708647
710.530878	97.263313	49.713652
707.248534	91.851464	49.718657
703.355431	92.268067	49.723661
699.668053	91.374281	49.728666
696.226063	91.517759	49.733671
692.416804	90.646226	49.738676
689.095198	96.424562	49.743681
685.532003	101.797804	49.748685
682.021345	94.662646	49.753690
678.714035	89.609064	49.758695
675.255955	98.800370	49.763700
672.352474	89.194118	49.768705
668.633194	91.997493	49.773709
664.528428	92.298562	49.778714
661.811775	91.319208	49.783719
657.548527	102.999974	49.788724
654.631474	95.480795	49.793729
650.767699	97.990426	49.798733
647.231138	92.314689	49.803738
643.870470	87.247332	49.808743
639.805308	93.404726	49.813748
636.396982	97.510357	49.818753
633.446290	91.913718	49.823757
630.201434	92.959667	49.828762
626.877792	93.508585	49.833767
623.052361	100.147306	49.838772
619.330266	89.805562	49.843777
616.000236	81.794254	49.848781
611.967862	93.362941	49.853786
608.541761	90.786262	49.858791
604.764467	93.617730	49.863796
601.657326	88.352494	49.868801
598.737538	89.246302	49.873805
595.116012	94.853337	49.878810
591.425658	87.407840	49.883815
587.345614	87.243158	49.888820
584.104532	84.836832	49.893825
580.533036	96.418774	49.898829
577.089811	93.515754	49.903834
574.099240	92.107921	49.908839
569.880730	92.866615	49.913844
566.736162	88.360237	49.918849
563.296809	90.442758	49.923853
559.435487	93.344352	49.928858
556.375877	83.389275	49.933863
552.906676	88.599138	49.938868
549.206961	99.957561	49.943873
545.912002	93.563812	49.948877
541.986772	94.567654	49.953882
538.753224	91.046508	49.958887
535.179387	99.287865	49.963892
531.879925	95.710604	49.968897
528.534334	88.916665	49.973901
524.205255	90.236869	49.978906
521.206477	89.453608	49.983911
517.124333	94.468417	49.988916
514.153091	89.520456	49.993921
510.672714	91.938456	49.998925
506.933331	89.932911	50.003930
503.878854	95.403707	50.008935
500.459193	90.155821	50.013940
496.729804	91.315672	50.018945
492.919143	85.926548	50.023949
489.548041	99.698114	50.028954
486.300397	84.435196	50.033959
482.804906	92.727572	50.038964
479.075527	91.318429	50.043969
475.381761	91.621649	50.048973
471.867298	96.803830	50.053978
468.812487	90.935655	50.058983
464.999365	96.278513	50.063988
462.071282	84.970917	50.068993
458.368095	88.224274	50.073997
454.573503	95.778887	50.079002
451.505108	93.139916	50.084007
447.180733	93.605196	50.089012
443.743813	92.004725	50.094017
440.180416	93.129108	50.099021
437.222417	93.013375	50.104026
433.894407	93.151754	50.109031
430.204582	99.516201	50.114036
426.567760	80.954327	50.119041
422.957466	92.770183	50.124045
419.464749	103.571035	50.129050
416.248336	88.929688	50.134055
412.742263	89.114948	50.139060
409.573952	96.346852	50.144065
405.662276	88.796902	50.149069
401.925868	96.443662	50.154074
398.552100	92.916060	50.159079
394.792312	99.940056	50.164084
391.627185	89.150513	50.169089
388.011438	92.984994	50.174093
384.187637	94.071093	50.179098
380.987174	93.341617	50.184103
377.468447	98.420093	50.189108
374.534398	97.591941	50.194113
370.694612	93.830458	50.199117
367.182008	86.607165	50.204122
363.673141	84.053041	50.209127
359.859298	95.366121	50.214132
356.530575	90.123034	50.219137
352.926554	95.199060	50.224141
349.608757	96.240715	50.229146
346.352769	82.580053	50.234151
342.173295	97.050925	50.239156
338.918658	85.016242	50.244161
334.945522	86.056150	50.249165
331.790660	93.162581	50.254170
328.375161	87.974229	50.259175
325.024371	90.175843	50.264180
321.728159	92.343599	50.269185
318.301525	94.329303	50.274189
314.612700	90.186692	50.279194
310.797378	93.717103	50.284199
307.337783	98.286463	50.289204
303.933035	95.197191	50.294209
300.649460	91.041726	50.299213
296.803749	87.028105	50.304218
293.957021	88.198470	50.309223
289.831462	83.333339	50.314228
286.236934	89.053313	50.319233
283.052868	84.062848	50.324237
279.522472	82.764992	50.329242
276.330804	96.847027	50.334247
272.075709	90.084939	50.339252
268.979264	79.572604	50.344257
265.354205	84.702575	50.349261
261.981471	89.204558	50.354266
258.469012	87.119281	50.359271
254.735895	79.025743	50.364276
251.787594	79.943111	50.369281
247.881492	91.827505	50.374285
244.090396	87.277001	50.379290
241.369060	89.946356	50.384295
237.846480	88.046173	50.389300
234.251690	85.489744	50.394305
230.357020	82.078617	50.399309
226.604186	93.483424	50.404314
223.211746	76.977813	50.409319
219.895714	84.277202	50.414324
216.450147	80.112350	50.419329
212.833712	80.678813	50.424333
209.124738	85.676417	50.429338
206.086809	81.953915	50.434343
202.188316	84.105332	50.439348
198.702670	86.103489	50.444353
195.459556	81.786705	50.449357
191.938941	87.919081	50.454362
188.523953	81.487344	50.459367
184.755667	75.667785	50.464372
181.347251	79.289524	50.469377
177.850606	78.090827	50.474381
174.649278	78.383466	50.479386
171.017867	71.871750	50.484391
166.736402	78.525127	50.489396
163.542044	75.535836	50.494401
160.435277	74.779109	50.499405
156.879848	86.852204	50.504410
153.464800	79.851013	50.509415
149.685602	86.504808	50.514420
146.378089	86.788781	50.519425
142.630895	83.949382	50.524429
138.840433	86.757788	50.529434
135.848323	81.284890	50.534439
132.453351	92.111638	50.539444
128.888769	90.294011	50.544449
125.263701	87.394357	50.549453
121.600810	87.610629	50.554458
118.237652	78.823279	50.559463
114.543050	81.853958	50.564468
111.143182	79.858674	50.569473
108.247115	82.068219	50.574477
104.191481	89.733458	50.579482
100.874273	82.245557	50.584487
97.452295	80.801076	50.589492
93.985836	82.710844	50.594497
90.345249	79.370710	50.599501
86.392056	89.936912	50.604506
83.161340	84.745027	50.609511
79.738374	88.691790	50.614516
76.369111	82.863549	50.619521
72.712987	84.904282	50.624525
69.229276	83.849138	50.629530
65.922932	81.769615	50.634535
62.690303	77.448081	50.639540
58.940996	83.806158	50.644545
55.318787	77.179158	50.649549
51.265343	88.048982	50.654554
47.976467	88.934355	50.659559
44.128004	84.620727	50.664564
41.032542	80.957922	50.669569
37.983776	83.637507	50.674573
34.437420	79.074070	50.679578
30.600081	77.052448	50.684583
27.276033	83.429330	50.689588
23.991904	76.499436	50.694593
20.684129	85.695862	50.699597
16.916688	80.252740	50.704602
13.208845	74.664242	50.709607
9.335588	90.055363	50.714612
5.536875	83.550951	50.719617
2.249591	78.747620	50.724621