Number of Data Points = 24
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3999_Position 115_00001.hld	3215.560438	296435.152126	622.055667	258370753.872927	3529.457195	3572.966336	34.288020	1.147325	0.000000	-31.637008	7.564096	-130.163000	-57.544500	-0.239334
3999_Position 115_00002.hld	3212.387700	294069.224677	602.433206	257867283.161836	3524.994105	3578.489562	33.238821	1.140390	0.000000	-33.641268	7.399848	-130.113000	-57.544500	-0.241161
3999_Position 115_00003.hld	3222.985970	297449.293557	644.054884	259551010.644391	3525.609736	3569.364789	35.419820	1.146015	0.000000	-32.464595	7.798895	-130.063000	-57.544500	-0.223311
3999_Position 115_00004.hld	3223.461730	293034.915979	625.448334	259626722.616054	3523.942808	3574.851565	34.391536	1.128678	0.000000	-33.850400	7.702347	-130.013000	-57.544500	-0.204062
3999_Position 115_00005.hld	3210.784447	297087.688806	602.139368	257613055.828526	3522.759935	3580.824637	33.238997	1.153232	0.000000	-34.659233	7.327888	-130.213000	-57.494500	-0.243069
3999_Position 115_00006.hld	3224.570905	321403.988942	712.285825	259803278.648524	3525.641571	3562.992622	39.153160	1.237105	0.000000	-32.165080	7.967480	-130.163000	-57.494500	-0.155011
3999_Position 115_00007.hld	3218.457168	310688.047936	658.447807	258830855.917797	3523.750720	3572.344042	36.261700	1.200352	0.000000	-34.397627	7.643845	-130.113000	-57.494500	-0.168111
3999_Position 115_00008.hld	3230.121756	308348.867816	686.867233	260687755.199039	3523.572410	3566.812225	37.691838	1.182828	0.000000	-33.122983	8.019091	-130.063000	-57.494500	-0.163720
3999_Position 115_00009.hld	3228.308498	299928.881626	665.206082	260398663.652322	3522.149362	3566.469359	36.523439	1.151807	0.000000	-33.150961	7.983524	-130.013000	-57.494500	-0.175246
3999_Position 115_00010.hld	3220.100281	318201.857585	684.442979	259092022.171215	3523.962015	3568.780011	37.674290	1.228142	0.000000	-33.707837	7.748847	-130.213000	-57.444500	-0.167458
3999_Position 115_00011.hld	3225.006261	314035.690109	680.936439	259872594.080934	3524.500053	3570.892828	37.424944	1.208422	0.000000	-33.888734	7.816395	-130.163000	-57.444500	-0.138281
3999_Position 115_00012.hld	3199.645192	292135.583482	558.104393	255850179.968554	3523.028915	3592.227100	30.914157	1.141823	0.000000	-38.414976	6.936085	-130.113000	-57.444500	-0.122722
3999_Position 115_00013.hld	3220.937341	308177.107916	656.456546	259225120.227387	3522.999235	3573.028933	36.124535	1.188840	0.000000	-35.409629	7.686434	-130.063000	-57.444500	-0.096144
3999_Position 115_00014.hld	3223.879020	307050.658477	666.794945	259693138.854709	3522.765703	3569.244556	36.660374	1.182360	0.000000	-17.912499	7.789914	-130.013000	-57.444500	-0.042226
3999_Position 115_00015.hld	3231.140450	334103.445094	761.102313	260850238.364527	3524.230896	3560.370278	41.752478	1.280825	0.000000	-32.704901	8.185183	-130.213000	-57.394500	-0.113480
3999_Position 115_00016.hld	3234.009974	334244.749314	773.399020	261308204.515005	3523.576248	3558.142221	42.389854	1.279121	0.000000	-32.247087	8.307695	-130.163000	-57.394500	-0.047066
3999_Position 115_00017.hld	3231.576946	320517.413486	724.567403	260919875.675795	3523.406616	3563.344645	39.742944	1.228413	0.000000	-33.102236	8.130192	-130.113000	-57.394500	-0.070646
3999_Position 115_00018.hld	3226.132210	315042.602321	692.203995	260051905.718935	3523.029664	3567.479491	38.031102	1.211460	0.000000	-34.269081	7.913675	-130.063000	-57.394500	-0.076835
3999_Position 115_00019.hld	3226.310058	313770.845965	684.223519	260080234.426115	3521.938446	3570.244647	37.590591	1.206439	0.000000	-35.092237	7.861968	-130.013000	-57.394500	-0.070521
3999_Position 115_00020.hld	3226.251407	324029.161846	710.165225	260070891.969801	3522.632701	3568.456098	39.016504	1.245926	0.000000	-34.114597	7.895649	-130.213000	-57.344500	-0.045595
3999_Position 115_00021.hld	3224.841160	315039.880134	682.694550	259846306.427491	3522.779414	3570.940174	37.523470	1.212409	0.000000	-34.186785	7.812346	-130.163000	-57.344500	-0.046512
3999_Position 115_00022.hld	3222.080171	323258.735369	700.827490	259406893.304456	3521.875953	3568.019871	38.552736	1.246146	0.000000	-29.112263	7.798611	-130.113000	-57.344500	-0.047500
3999_Position 115_00023.hld	3222.066534	318732.193653	688.282803	259404723.934697	3521.799045	3569.378924	37.862807	1.228706	0.000000	-35.090417	7.783632	-130.063000	-57.344500	-0.074699
3999_Position 115_00024.hld	3203.124495	296186.436957	576.608422	256400155.442331	3523.207813	3588.376980	31.904847	1.155173	0.000000	-38.823797	7.061345	-130.013000	-57.344500	-0.048487