Thu Aug 25 10:19:35 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
1.467575	102.444898	0.000000
1.522402	102.952055	0.005005
1.716594	93.968249	0.010010
1.480104	92.575340	0.015014
1.309321	86.141763	0.020019
1.152876	79.734417	0.025024
1.081789	69.039467	0.030029
0.766585	67.427939	0.035034
0.323140	59.701990	0.040038
-0.006881	47.674557	0.045043
-0.100834	49.726787	0.050048
-0.505983	39.735930	0.055053
-0.660488	28.168226	0.060058
-0.679074	24.064652	0.065062
-0.949560	18.273144	0.070067
-1.188750	18.858004	0.075072
-1.563750	13.902282	0.080077
-2.264628	-1.569274	0.085082
-2.492147	-3.972814	0.090086
-2.420542	-3.183552	0.095091
-2.604906	-10.292006	0.100096
-2.944519	-6.552983	0.105101
-2.992690	-9.959054	0.110106
-4.628998	-4.491938	0.115110
-4.009794	-2.478687	0.120115
-4.306969	-8.430520	0.125120
-4.888503	-7.687617	0.130125
-5.092940	-4.846129	0.135130
-4.901427	-4.414175	0.140134
-5.429336	-9.823656	0.145139
-5.202120	-10.330599	0.150144
-5.739576	-10.565871	0.155149
-6.275133	-3.243267	0.160154
-6.497010	-3.214774	0.165158
-6.436556	-14.610487	0.170163
-6.639593	-7.925277	0.175168
-6.687642	-3.861780	0.180173
-7.540190	-13.026373	0.185178
-8.042377	-2.611697	0.190182
-8.106915	-9.049231	0.195187
-8.169971	-1.101473	0.200192
-7.902054	-9.552615	0.205197
-8.173431	-10.114314	0.210202
-8.939626	-1.566006	0.215206
-9.329042	-15.998023	0.220211
-9.564344	-7.102632	0.225216
-9.855586	-4.769561	0.230221
-9.444004	-4.985853	0.235226
-9.887139	-8.573648	0.240230
-9.942762	-7.138031	0.245235
-10.543096	2.111950	0.250240
-11.094337	-5.220594	0.255245
-11.040807	-9.623359	0.260250
-11.236981	-8.301761	0.265254
-11.725764	-5.184768	0.270259
-12.176408	-7.664077	0.275264
-12.278312	-5.120228	0.280269
-12.620586	-5.019087	0.285274
-12.462880	-7.239377	0.290278
-12.547581	-6.757817	0.295283
-13.297422	-9.892597	0.300288
-14.149042	-2.650184	0.305293
-13.495014	-9.092738	0.310298
-13.990745	-0.207159	0.315302
-14.106970	-4.785806	0.320307
-14.190293	2.364702	0.325312
-14.189305	0.238569	0.330317
-14.393064	-2.538851	0.335322
-15.184383	-2.803948	0.340326
-15.130291	-7.690854	0.345331
-15.242660	-0.703474	0.350336
-15.724700	2.868043	0.355341
-16.137814	-6.115469	0.360346
-16.604134	-2.922902	0.365350
-16.710013	-4.203390	0.370355
-16.617439	-0.171416	0.375360
-16.871148	-2.207022	0.380365
-17.521411	-6.996221	0.385370
-17.912258	-6.536295	0.390374
-18.153543	-3.217636	0.395379
-18.088474	-5.860007	0.400384
-18.242030	2.548019	0.405389
-18.074543	-10.247021	0.410394
-18.975078	-10.289362	0.415398
-19.250149	-9.857067	0.420403
-19.814984	-9.012377	0.425408
-20.048004	-9.368115	0.430413
-19.846250	-9.317414	0.435418
-19.933269	-3.121778	0.440422
-19.956826	0.365246	0.445427
-20.366722	-13.965486	0.450432
-21.013395	0.644800	0.455437
-21.158015	-4.745643	0.460442
-21.796386	1.833775	0.465446
-21.097159	-4.682302	0.470451
-22.044529	-3.973825	0.475456
-22.630435	-1.445888	0.480461
-22.738432	-2.124933	0.485466
-23.073185	-0.538013	0.490470
-22.877926	-6.563838	0.495475
-22.785129	-8.337361	0.500480
-22.545072	6.336470	0.505485
-22.942585	-8.976965	0.510490
-23.773235	-6.752363	0.515494
-23.713051	-12.905718	0.520499
-24.514963	-4.114535	0.525504
-25.288689	2.922688	0.530509
-25.628859	-7.135268	0.535514
-25.690714	-1.579487	0.540518
-25.477318	2.376609	0.545523
-25.054763	-0.793173	0.550528
-25.665424	-5.063396	0.555533
-25.883456	-11.179486	0.560538
-26.624573	-2.103600	0.565542
-26.839116	-5.559533	0.570547
-26.890341	-3.058425	0.575552
-27.157519	-3.826424	0.580557
-26.827205	-10.126508	0.585562
-27.276472	1.842764	0.590566
-27.958863	-9.721293	0.595571
-28.472011	-7.900778	0.600576
-28.838436	1.154365	0.605581
-28.759445	-10.063920	0.610586
-29.080887	2.828118	0.615590
-28.513859	6.023291	0.620595
-29.530016	5.603600	0.625600
-30.101025	0.868420	0.630605
-29.984326	-8.027261	0.635610
-30.321706	0.767068	0.640614
-30.330349	3.340598	0.645619
-30.233782	7.511152	0.650624
-30.469278	3.780091	0.655629
-30.934862	-9.421953	0.660634
-31.463966	-5.441268	0.665638
-31.716853	-4.797314	0.670643
-31.779269	-3.468200	0.675648
-32.114775	-1.200958	0.680653
-32.919925	-3.210270	0.685658
-33.230129	-1.215911	0.690662
-33.143191	-3.061282	0.695667
-33.003876	4.269476	0.700672
-33.600836	-2.723710	0.705677
-32.974771	-5.412853	0.710682
-33.340978	-5.127629	0.715686
-34.467399	0.237454	0.720691
-34.413022	1.193930	0.725696
-34.889550	-5.732704	0.730701
-34.603670	-1.784804	0.735706
-34.736939	4.620560	0.740710
-35.581296	-1.400559	0.745715
-35.981086	4.170210	0.750720
-36.125939	1.196900	0.755725
-35.845622	0.419046	0.760730
-36.390725	-6.408258	0.765734
-36.744759	-7.327162	0.770739
-36.938751	-9.460707	0.775744
-37.498349	1.788701	0.780749
-37.534249	1.699469	0.785754
-37.832397	3.366075	0.790758
-37.406942	-3.515228	0.795763
-37.408693	-2.733454	0.800768
-38.320057	1.076174	0.805773
-38.496576	-4.090972	0.810778
-39.195514	3.598918	0.815782
-39.092695	-2.387114	0.820787
-39.416692	-1.054978	0.825792
-40.244463	5.620557	0.830797
-40.377227	0.959079	0.835802
-40.551863	-1.117389	0.840806
-40.801947	3.366906	0.845811
-40.480428	-0.808933	0.850816
-40.944498	4.427060	0.855821
-40.400853	-4.573485	0.860826
-40.799135	6.353258	0.865830
-41.187618	4.750056	0.870835
-41.731669	2.275892	0.875840
-42.316245	9.758041	0.880845
-42.683719	-0.235528	0.885850
-43.214773	2.141449	0.890854
-43.621235	5.669487	0.895859
-42.959332	-0.878708	0.900864
-43.576201	6.526243	0.905869
-43.189400	-9.371987	0.910874
-43.520790	-1.163889	0.915878
-44.227772	-0.689228	0.920883
-44.585470	3.606285	0.925888
-44.906710	6.510369	0.930893
-44.757370	3.196735	0.935898
-44.907153	0.031210	0.940902
-45.568548	8.275201	0.945907
-45.842989	3.882694	0.950912
-46.398271	7.408741	0.955917
-45.909806	-2.829672	0.960922
-46.398853	13.840829	0.965926
-46.249962	5.212180	0.970931
-46.761849	-1.601347	0.975936
-47.516761	7.388121	0.980941
-47.323863	-2.101631	0.985946
-47.927816	-3.370514	0.990950
-48.147058	-2.946966	0.995955
-47.579646	-2.346123	1.000960
-48.632970	2.175445	1.005965
-48.911795	2.491271	1.010970
-49.025526	8.172242	1.015974
-49.188140	-1.657273	1.020979
-49.298245	2.124885	1.025984
-49.540096	1.087164	1.030989
-49.651904	-4.571009	1.035994
-50.474048	1.429766	1.040998
-50.554762	5.748318	1.046003
-50.674555	5.352694	1.051008
-50.996114	11.698978	1.056013
-50.855183	2.495776	1.061018
-51.356889	17.314312	1.066022
-52.010925	8.741869	1.071027
-51.944682	5.871523	1.076032
-52.524665	8.942699	1.081037
-52.226729	10.778497	1.086042
-52.290675	3.831507	1.091046
-52.773457	-2.059603	1.096051
-53.287252	-7.806648	1.101056
-53.996776	0.821366	1.106061
-53.844818	-5.172363	1.111066
-53.891642	-1.824063	1.116070
-53.976657	4.674979	1.121075
-54.670421	3.844109	1.126080
-55.430391	10.806413	1.131085
-54.883885	4.782496	1.136090
-55.105336	3.216399	1.141094
-55.221648	-1.137609	1.146099
-55.078214	-0.150795	1.151104
-55.745646	5.461910	1.156109
-55.963527	-0.458053	1.161114
-56.257927	-2.803654	1.166118
-56.816844	-6.294211	1.171123
-57.295231	1.101694	1.176128
-57.920412	1.240837	1.181133
-57.611355	2.875576	1.186138
-58.150458	-0.836384	1.191142
-58.382215	2.585186	1.196147
-58.267831	-0.428742	1.201152
-58.207726	10.685605	1.206157
-57.924610	-0.251457	1.211162
-58.338711	5.555671	1.216166
-59.195122	7.790640	1.221171
-59.470381	5.502149	1.226176
-59.817110	-2.232592	1.231181
-59.901664	-4.788244	1.236186
-60.537360	5.906781	1.241190
-61.147280	4.021903	1.246195
-61.043294	-1.752340	1.251200
-61.115275	2.666082	1.256205
-61.061515	2.271738	1.261210
-61.352632	-1.912510	1.266214
-61.450969	0.402991	1.271219
-61.396035	-6.407598	1.276224
-62.091598	1.980949	1.281229
-62.217146	-3.162546	1.286234
-62.229625	-2.334799	1.291238
-63.223159	-2.033535	1.296243
-63.498046	-3.983562	1.301248
-63.933004	3.949701	1.306253
-63.600693	-3.473825	1.311258
-63.675016	-4.645362	1.316262
-63.626924	1.798021	1.321267
-64.831139	-1.123190	1.326272
-65.190550	1.752073	1.331277
-64.981277	-3.051580	1.336282
-65.178179	-9.158324	1.341286
-65.202702	2.054699	1.346291
-65.477448	0.041374	1.351296
-66.160526	0.404724	1.356301
-66.404642	-2.483428	1.361306
-66.505773	6.068241	1.366310
-66.530968	0.424970	1.371315
-66.982193	-7.913488	1.376320
-67.122114	-0.149841	1.381325
-67.367172	-1.364228	1.386330
-67.799963	2.038222	1.391334
-68.266265	-5.475302	1.396339
-68.003958	-8.224507	1.401344
-68.406380	0.817293	1.406349
-68.678254	-12.282218	1.411354
-69.452981	-6.526154	1.416358
-69.522029	-1.329913	1.421363
-69.655785	-2.893932	1.426368
-69.624722	-3.291047	1.431373
-69.863725	-4.620277	1.436378
-69.766930	-4.157664	1.441382
-70.469245	6.446559	1.446387
-71.052518	-3.703014	1.451392
-71.378436	9.502937	1.456397
-71.470086	1.022712	1.461402
-71.406055	-7.285750	1.466406
-71.617260	-11.963405	1.471411
-71.670910	-5.659107	1.476416
-72.495068	-7.001051	1.481421
-72.671027	-5.302971	1.486426
-72.786475	-2.798128	1.491430
-73.109142	-0.156412	1.496435
-72.999657	-12.445649	1.501440
-73.383284	-8.427648	1.506445
-73.774797	-5.765654	1.511450
-73.868741	-6.228603	1.516454
-74.089196	-3.106196	1.521459
-74.087084	-13.474038	1.526464
-74.820140	-2.589758	1.531469
-75.274728	-15.508776	1.536474
-75.448308	-6.360469	1.541478
-75.549521	2.577187	1.546483
-75.520325	-14.641228	1.551488
-76.242328	-5.726525	1.556493
-76.163431	-8.228694	1.561498
-76.720121	-7.704814	1.566502
-77.619764	-4.909416	1.571507
-77.411930	-3.866256	1.576512
-77.570498	0.527768	1.581517
-77.322596	-4.911521	1.586522
-77.281021	-5.993651	1.591526
-77.358127	2.263188	1.596531
-78.151163	1.030262	1.601536
-78.484704	1.028796	1.606541
-78.793310	-3.665236	1.611546
-79.083222	-6.350059	1.616550
-78.972063	0.915504	1.621555
-79.352829	-0.549700	1.626560
-79.962887	-2.893295	1.631565
-80.150029	-4.078791	1.636570
-80.436462	-5.368951	1.641574
-80.733260	-1.984647	1.646579
-80.666258	3.456031	1.651584
-80.892868	2.631058	1.656589
-81.430031	-1.188771	1.661594
-82.030977	0.844820	1.666598
-82.064248	-1.380347	1.671603
-81.948977	-9.408937	1.676608
-82.122152	4.295092	1.681613
-82.089514	-6.213577	1.686618
-82.657743	-4.523633	1.691622
-83.630500	-6.275724	1.696627
-83.402580	-7.627496	1.701632
-83.260123	-3.552723	1.706637
-83.518961	-18.058970	1.711642
-83.641062	-3.733366	1.716646
-84.714167	-1.214506	1.721651
-84.661518	-1.539074	1.726656
-85.138776	-4.397021	1.731661
-85.364803	-6.269282	1.736666
-85.128849	-5.815820	1.741670
-85.656672	-6.027286	1.746675
-85.134316	-3.423067	1.751680
-86.116828	1.191812	1.756685
-86.217268	-4.357410	1.761690
-86.375099	5.212375	1.766694
-86.546658	-4.324668	1.771699
-86.904983	-12.639713	1.776704
-87.868111	-3.206339	1.781709
-88.252208	-7.394997	1.786714
-87.768175	-3.841980	1.791718
-87.941834	-8.107904	1.796723
-87.585117	-3.085946	1.801728
-88.105825	-4.345724	1.806733
-88.799979	-9.393790	1.811738
-89.101042	-2.591982	1.816742
-89.375131	-0.603280	1.821747
-89.423791	-13.155635	1.826752
-89.503146	-1.032361	1.831757
-90.308165	-2.605091	1.836762
-90.652946	-1.171622	1.841766
-91.155008	0.115652	1.846771
-90.729893	-1.827002	1.851776
-91.151319	2.393076	1.856781
-91.242683	-8.349260	1.861786
-91.211325	-2.172176	1.866790
-91.732002	3.806674	1.871795
-91.828100	-3.891406	1.876800
-92.228603	-3.297086	1.881805
-92.315616	-3.688355	1.886810
-92.688433	0.195077	1.891814
-93.565743	-1.704846	1.896819
-93.374845	-4.395406	1.901824
-93.944077	-1.167728	1.906829
-93.637480	-5.005872	1.911834
-93.947757	-7.807725	1.916838
-93.992718	-9.233797	1.921843
-94.633216	-4.125184	1.926848
-95.030450	1.824831	1.931853
-95.555875	-6.229915	1.936858
-95.305372	-5.892627	1.941862
-95.503755	7.619201	1.946867
-95.403481	-7.465339	1.951872
-95.733172	-0.763448	1.956877
-96.524383	-3.031200	1.961882
-96.677671	-3.813878	1.966886
-97.120177	-4.826483	1.971891
-96.598117	0.017708	1.976896
-96.806320	-1.294201	1.981901
-97.768009	-1.488302	1.986906
-98.105542	3.674080	1.991910
-98.628480	5.217724	1.996915
-98.665890	-2.462170	2.006912
-97.385206	4.920952	2.016909
-97.787050	-1.959764	2.026906
-97.628994	-0.698298	2.036902
-96.647903	1.609453	2.046899
-95.773770	-9.158504	2.056896
-95.632703	-8.641974	2.066893
-95.016765	-6.650805	2.076890
-94.735756	-2.098266	2.086886
-94.164333	1.363397	2.096883
-93.366291	-4.359023	2.106880
-93.213373	-6.749211	2.116877
-92.753732	-7.793634	2.126874
-91.841018	-2.871247	2.136870
-91.928627	-5.340954	2.146867
-90.796347	-1.704247	2.156864
-90.201513	-9.241645	2.166861
-90.096508	-1.439887	2.176858
-89.937939	-2.262906	2.186854
-89.198656	-7.906426	2.196851
-88.645738	-4.270803	2.206848
-87.474916	-11.654533	2.216845
-87.418705	-14.837353	2.226842
-87.480977	-2.818402	2.236838
-87.058547	-5.086096	2.246835
-86.179917	-11.793652	2.256832
-85.298012	-6.498974	2.266829
-84.448303	-6.261375	2.276826
-84.752855	-8.202915	2.286822
-84.522512	-4.114437	2.296819
-83.415840	-4.161022	2.306816
-83.015188	-2.513085	2.316813
-82.568678	-6.403292	2.326810
-81.930807	-4.459907	2.336806
-81.745318	1.878395	2.346803
-80.986245	-2.656333	2.356800
-80.398723	-0.119018	2.366797
-80.324644	3.198832	2.376794
-79.269082	2.948014	2.386790
-78.872052	-0.148829	2.396787
-79.026102	3.876338	2.406784
-77.504180	-2.963697	2.416781
-77.239011	1.271379	2.426778
-77.295174	-5.685678	2.436774
-76.763574	-1.793290	2.446771
-76.016273	-2.255564	2.456768
-75.652881	-3.018811	2.466765
-74.929442	2.661830	2.476762
-74.258273	-2.448333	2.486758
-74.496059	-1.178694	2.496755
-73.454913	-4.474665	2.506752
-73.162078	-4.324036	2.516749
-72.577111	-3.595127	2.526746
-71.599696	-3.751337	2.536742
-71.663512	-5.483511	2.546739
-71.140856	-2.109238	2.556736
-70.310157	-6.816745	2.566733
-70.412560	-4.694009	2.576730
-69.841177	-5.081201	2.586726
-69.136156	-3.680526	2.596723
-67.883243	1.112533	2.606720
-67.875408	-7.571494	2.616717
-67.428346	-0.488566	2.626714
-67.082665	-1.388420	2.636710
-66.646543	-0.078657	2.646707
-66.084647	-3.977441	2.656704
-65.708477	3.826181	2.666701
-65.028484	1.071471	2.676698
-64.819855	2.648129	2.686694
-63.870880	-0.579547	2.696691
-63.416815	-5.769731	2.706688
-63.263732	-5.654225	2.716685
-62.119463	-4.537784	2.726682
-61.752215	0.330695	2.736678
-61.793065	4.759441	2.746675
-60.958266	1.581333	2.756672
-60.556606	2.376979	2.766669
-60.378213	-3.742522	2.776666
-59.592117	2.593538	2.786662
-59.106948	4.681229	2.796659
-58.037658	0.794807	2.806656
-57.717382	-8.435519	2.816653
-57.614391	-6.965853	2.826650
-57.138493	0.166410	2.836646
-56.367773	4.262085	2.846643
-56.083946	4.258905	2.856640
-55.490757	-3.633030	2.866637
-54.564654	-2.190967	2.876634
-54.387200	3.869831	2.886630
-54.331621	2.613124	2.896627
-53.557737	-6.457031	2.906624
-53.207283	4.803513	2.916621
-52.406091	4.589388	2.926618
-51.807717	0.928808	2.936614
-51.781461	10.507372	2.946611
-50.873557	-2.644892	2.956608
-50.330965	-1.507033	2.966605
-50.168259	0.824420	2.976602
-49.430080	2.948494	2.986598
-48.900400	-1.600975	2.996595
-48.513454	9.162847	3.006592
-47.581569	4.255752	3.016589
-47.068171	1.191360	3.026586
-46.952309	5.019015	3.036582
-46.930825	8.918478	3.046579
-45.824719	-0.495171	3.056576
-45.533723	3.419082	3.066573
-44.885682	-3.046438	3.076570
-44.472709	3.924627	3.086566
-44.220746	1.214810	3.096563
-43.219459	5.277529	3.106560
-42.496718	-0.908260	3.116557
-42.714274	-1.795888	3.126554
-41.970883	4.112880	3.136550
-41.468306	-3.438574	3.146547
-41.240995	0.922812	3.156544
-40.477959	-4.572375	3.166541
-40.073754	-0.631512	3.176538
-39.029163	3.278703	3.186534
-38.643529	4.700916	3.196531
-38.442509	2.683324	3.206528
-38.142616	-6.455112	3.216525
-37.665509	-4.860333	3.226522
-37.085796	-8.416617	3.236518
-36.159120	0.206737	3.246515
-35.367768	-1.196934	3.256512
-35.453426	5.136341	3.266509
-35.403341	1.583846	3.276506
-34.816549	1.466671	3.286502
-34.201378	2.704033	3.296499
-33.080707	2.474697	3.306496
-32.471549	-3.547575	3.316493
-32.444674	-3.564347	3.326490
-32.361943	-3.577199	3.336486
-31.431646	-1.936220	3.346483
-31.069225	-4.878752	3.356480
-29.967548	-2.250933	3.366477
-29.793614	-0.681509	3.376474
-29.788944	7.044112	3.386470
-29.052219	-4.063446	3.396467
-28.346277	-1.633379	3.406464
-27.881529	-1.645900	3.416461
-26.993426	-2.849320	3.426458
-26.883501	-1.060793	3.436454
-26.511508	-3.830597	3.446451
-26.180267	-6.581344	3.456448
-25.423261	1.602933	3.466445
-24.905837	-5.105047	3.476442
-24.217717	-0.666976	3.486438
-23.883506	-4.203800	3.496435
-23.373049	-2.759964	3.506432
-22.889277	1.447200	3.516429
-22.339941	-5.167579	3.526426
-22.083416	-7.079826	3.536422
-21.224313	-4.483689	3.546419
-20.669269	-0.632982	3.556416
-20.499682	-5.794431	3.566413
-20.261307	-10.858952	3.576410
-19.585905	-6.684984	3.586406
-18.938742	-4.784231	3.596403
-18.338871	-0.937379	3.606400
-17.865692	-3.608997	3.616397
-17.106321	-7.164921	3.626394
-16.775215	-0.820921	3.636390
-16.461430	-7.655382	3.646387
-15.873934	-5.418997	3.656384
-15.008754	-11.703127	3.666381
-15.008446	-2.114164	3.676378
-14.633791	0.773289	3.686374
-13.653059	2.507738	3.696371
-13.450483	-8.357736	3.706368
-13.240371	-2.127825	3.716365
-12.465725	-2.100203	3.726362
-11.748761	-3.789989	3.736358
-10.979868	1.322839	3.746355
-10.606794	-1.618195	3.756352
-10.700791	-1.574847	3.766349
-10.138840	-5.685879	3.776346
-9.465044	-4.448198	3.786342
-8.621317	-2.296309	3.796339
-8.000983	-1.778843	3.806336
-7.533026	4.755959	3.816333
-7.551001	-1.845959	3.826330
-7.324177	0.998134	3.836326
-6.445090	-2.570211	3.846323
-6.048135	-2.644968	3.856320
-5.300341	-0.322825	3.866317
-4.984105	4.062645	3.876314
-4.516978	7.553330	3.886310
-3.861586	11.755783	3.896307
-3.760312	16.716630	3.906304
-3.214064	30.968595	3.916301
-2.758124	32.180226	3.926298
-2.093348	46.578358	3.936294
-1.662565	61.222240	3.946291
-1.300947	67.932118	3.956288
-0.903856	85.837802	3.966285
-0.353410	93.427264	3.976282
-0.024737	120.780606	3.986278
0.000000	125.621486	3.991283
0.396803	141.080796	3.996288
0.932274	148.232485	4.001293
1.005539	154.058212	4.006298
1.090080	166.247678	4.011302
1.475717	179.842148	4.016307
1.421179	171.175686	4.021312
1.726895	160.405825	4.026317
1.548843	181.362122	4.031322
1.445503	167.916522	4.036326
1.248846	181.744597	4.041331
1.251940	179.048634	4.046336
1.762590	175.444237	4.051341
1.582232	182.163930	4.056346
1.515258	179.950347	4.061350
1.731597	183.004348	4.066355
1.382829	187.475677	4.071360
1.666381	184.621874	4.076365
1.598389	188.084259	4.081370
2.082448	181.117773	4.086374
1.721745	183.967955	4.091379
1.611583	164.246501	4.096384
1.666629	155.746376	4.101389
1.472617	168.140840	4.106394
1.488133	161.804597	4.111398
1.648096	168.803159	4.116403
1.501970	183.309856	4.121408
1.930621	175.349138	4.126413
1.861161	171.253501	4.131418
1.631158	172.093192	4.136422
1.552852	177.977476	4.141427
1.726950	188.406524	4.146432
1.806997	177.883983	4.151437
1.372423	181.754983	4.156442
1.868658	182.778280	4.161446
1.935718	184.735695	4.166451
1.672426	181.255725	4.171456
1.844683	179.086916	4.176461
1.529995	186.080759	4.181466
2.106152	174.626270	4.186470
1.828878	180.260155	4.191475
1.891226	181.360925	4.196480
1.567407	187.767738	4.201485
1.753252	181.771798	4.206490
2.312505	174.565741	4.211494
2.124969	190.072357	4.216499
2.000015	181.084728	4.221504
1.846422	178.824605	4.226509
1.689370	181.984566	4.231514
1.798532	184.558648	4.236518
1.848712	177.865789	4.241523
1.701992	184.564393	4.246528
1.932120	177.606057	4.251533
1.884802	181.489148	4.256538
2.065137	179.657597	4.261542
1.522552	185.358363	4.266547
1.226836	186.967656	4.271552
2.044415	194.736392	4.276557
2.111945	202.179723	4.281562
2.240645	217.940537	4.286566
2.692516	208.739127	4.291571
1.916029	204.801718	4.296576
1.921765	198.106325	4.301581
2.041929	211.448182	4.306586
2.604492	207.905248	4.311590
2.267334	197.293040	4.316595
2.033013	189.205236	4.321600
2.346302	185.138211	4.326605
2.115756	183.636795	4.331610
2.067551	178.582367	4.336614
1.930890	185.298379	4.341619
2.128580	207.660662	4.346624
2.433313	208.498828	4.351629
2.102113	216.599429	4.356634
2.323263	213.676304	4.361638
2.316454	216.863351	4.366643
2.022948	217.263737	4.371648
2.840816	212.465910	4.376653
2.726233	219.577111	4.381658
2.334379	197.764205	4.386662
2.020525	198.806861	4.391667
2.228957	212.321552	4.396672
2.520383	203.145284	4.401677
2.544370	208.143513	4.406682
2.654616	209.834735	4.411686
2.335180	196.764658	4.416691
2.422430	191.113196	4.421696
2.265369	185.079233	4.426701
2.475632	207.357288	4.431706
2.711155	208.674538	4.436710
2.518240	215.873941	4.441715
2.339620	203.050718	4.446720
2.690437	197.826196	4.451725
2.377253	207.594444	4.456730
2.367627	199.066466	4.461734
2.287299	206.637369	4.466739
2.785067	205.028165	4.471744
2.655864	203.251439	4.476749
2.477383	212.425940	4.481754
2.511617	203.141272	4.486758
2.595017	208.832550	4.491763
2.315896	223.942254	4.496768
2.654470	212.145313	4.501773
2.510935	212.901854	4.506778
2.741575	220.129809	4.511782
2.733890	209.646305	4.516787
2.826760	218.246779	4.521792
2.812756	201.338636	4.526797
2.933355	215.094883	4.531802
2.736688	209.449935	4.536806
2.410791	210.586228	4.541811
2.741491	212.825044	4.546816
2.545102	211.122120	4.551821
2.355904	202.533690	4.556826
2.480896	206.434081	4.561830
2.777174	210.045041	4.566835
2.459424	214.378638	4.571840
2.800889	211.151922	4.576845
2.497323	218.175673	4.581850
2.415450	214.486935	4.586854
3.232273	220.778317	4.591859
2.765999	230.855303	4.596864
2.755382	218.739743	4.601869
2.667209	230.219154	4.606874
3.001042	239.044476	4.611878
2.870905	239.564800	4.616883
2.936894	241.095278	4.621888
3.032943	241.194180	4.626893
2.618516	246.321223	4.631898
3.192081	238.128962	4.636902
3.279321	244.920646	4.641907
3.021007	247.545986	4.646912
2.956593	234.641571	4.651917
2.730226	236.989819	4.656922
2.961927	237.383845	4.661926
2.954188	249.499241	4.666931
3.035333	242.779360	4.671936
3.113167	243.324046	4.676941
2.970976	241.176025	4.681946
3.215016	241.954100	4.686950
2.801388	245.053032	4.691955
3.104608	237.352386	4.696960
3.103861	241.266158	4.701965
2.860100	240.918425	4.706970
3.035830	238.445342	4.711974
3.301472	245.069868	4.716979
3.275471	245.728901	4.721984
3.585348	235.853693	4.726989
3.161917	240.564526	4.731994
2.916964	244.098942	4.736998
3.288641	240.209420	4.742003
3.086830	242.066599	4.747008
3.368406	239.314338	4.752013
3.201197	240.508028	4.757018
3.280964	236.759157	4.762022
3.154189	229.698532	4.767027
2.741305	235.594129	4.772032
3.038621	239.271373	4.777037
2.943314	241.029605	4.782042
3.359172	251.164543	4.787046
3.433024	251.320708	4.792051
3.607908	256.966030	4.797056
3.319907	248.709437	4.802061
3.323309	251.179876	4.807066
3.199490	253.629118	4.812070
3.706665	260.411960	4.817075
3.447177	262.385747	4.822080
3.659902	245.255375	4.827085
3.131055	253.029452	4.832090
3.464766	258.887173	4.837094
3.624345	255.518103	4.842099
3.536668	251.441121	4.847104
3.642824	244.821725	4.852109
3.290597	249.777671	4.857114
3.408521	256.463311	4.862118
3.728939	264.490310	4.867123
3.395796	272.404577	4.872128
3.451923	271.595399	4.877133
3.243031	265.765685	4.882138
3.639206	272.856992	4.887142
3.835170	268.688108	4.892147
3.787797	266.253141	4.897152
3.829086	270.489367	4.902157
3.921806	272.964797	4.907162
3.779703	258.645668	4.912166
3.541350	243.623452	4.917171
3.305383	251.032097	4.922176
3.667453	251.579705	4.927181
3.466536	272.210658	4.932186
3.525725	265.706182	4.937190
3.987987	262.716797	4.942195
3.466305	260.871845	4.947200
3.439643	263.280556	4.952205
3.645603	269.749925	4.957210
3.101903	268.889196	4.962214
3.511243	269.568605	4.967219
3.443849	275.476522	4.972224
3.795329	274.927956	4.977229
3.597257	285.798191	4.982234
3.788438	295.050858	4.987238
4.160242	292.838115	4.992243
4.100683	289.500210	4.997248
4.012601	282.164579	5.002253
3.772122	273.321556	5.007258
3.670085	270.331999	5.012262
3.727649	281.000825	5.017267
4.302899	288.295037	5.022272
4.291683	279.947605	5.027277
3.947698	278.698075	5.032282
3.887547	269.263645	5.037286
4.000545	269.521245	5.042291
3.677996	275.953200	5.047296
4.387181	276.696362	5.052301
4.134303	271.658157	5.057306
3.810397	273.091539	5.062310
3.877653	272.302764	5.067315
3.590995	282.563611	5.072320
4.213915	287.047235	5.077325
3.669415	286.711820	5.082330
4.343617	283.736681	5.087334
4.280812	296.958573	5.092339
4.227485	298.292613	5.097344
4.330751	296.169402	5.102349
4.340645	303.004866	5.107354
4.103840	292.168066	5.112358
4.239621	283.060438	5.117363
4.137579	296.361244	5.122368
4.105910	291.006797	5.127373
4.190107	300.032616	5.132378
4.219482	297.680534	5.137382
4.316428	294.058676	5.142387
4.106771	297.682486	5.147392
4.153422	294.407034	5.152397
4.215112	298.323691	5.157402
4.434843	297.814749	5.162406
4.255792	296.988634	5.167411
4.296692	304.572223	5.172416
4.400365	301.205577	5.177421
4.310404	305.766100	5.182426
4.199448	297.481745	5.187430
4.461527	293.457521	5.192435
4.498639	300.905659	5.197440
4.434692	289.851950	5.202445
4.139259	293.884673	5.207450
4.158758	283.868272	5.212454
4.233778	295.825198	5.217459
4.452042	304.674988	5.222464
4.695955	296.499549	5.227469
4.002090	305.299263	5.232474
4.288180	290.093595	5.237478
4.393709	292.225331	5.242483
4.203801	299.617288	5.247488
4.351531	292.529447	5.252493
4.198641	305.996416	5.257498
4.374564	303.570752	5.262502
4.544309	292.078624	5.267507
4.175482	300.245269	5.272512
4.873001	310.614524	5.277517
4.958058	313.850471	5.282522
4.510682	310.111412	5.287526
4.401525	299.086927	5.292531
4.426732	301.642542	5.297536
4.820939	319.744183	5.302541
4.572245	319.830662	5.307546
4.384391	333.398044	5.312550
5.041730	327.739475	5.317555
4.494635	327.879035	5.322560
5.154371	327.709282	5.327565
4.932663	316.234179	5.332570
4.798569	301.534105	5.337574
4.657660	302.603454	5.342579
4.257791	301.312058	5.347584
4.576338	306.014222	5.352589
4.718195	311.958969	5.357594
5.070684	322.891662	5.362598
5.181012	316.711354	5.367603
4.699536	310.914842	5.372608
4.449318	299.700484	5.377613
4.655766	310.978759	5.382618
4.603479	315.372028	5.387622
4.768115	322.025064	5.392627
4.647354	316.643438	5.397632
4.809721	315.624622	5.402637
4.767453	324.613320	5.407642
4.494044	321.011519	5.412646
4.889039	312.261900	5.417651
4.748290	324.578523	5.422656
4.920712	317.372907	5.427661
5.035806	325.650406	5.432666
4.555541	324.501321	5.437670
4.559189	321.982422	5.442675
4.570304	341.371662	5.447680
4.770517	337.701976	5.452685
4.922759	356.290826	5.457690
4.955078	351.264862	5.462694
5.239857	354.320824	5.467699
5.024613	350.482110	5.472704
5.034162	342.371844	5.477709
4.947132	352.636255	5.482714
4.941671	350.555384	5.487718
4.723339	346.040100	5.492723
4.477430	354.693720	5.497728
4.949727	352.629742	5.502733
4.775339	364.967483	5.507738
5.175442	364.208813	5.512742
5.376861	366.483723	5.517747
5.005673	379.152871	5.522752
5.311547	369.578778	5.527757
5.348501	373.274697	5.532762
5.565838	367.488900	5.537766
5.435107	363.409147	5.542771
5.005445	358.727652	5.547776
5.264135	348.629445	5.552781
4.910404	351.877200	5.557786
5.321729	357.377939	5.562790
5.593223	366.440886	5.567795
5.426080	363.002763	5.572800
5.269070	341.225652	5.577805
5.291767	350.302263	5.582810
5.385014	353.008579	5.587814
5.399681	355.439301	5.592819
5.184636	363.626174	5.597824
5.140985	359.102500	5.602829
5.434398	373.806244	5.607834
5.447718	369.507764	5.612838
5.500191	367.655099	5.617843
5.533244	369.728596	5.622848
5.587973	374.930865	5.627853
5.059903	373.428593	5.632858
5.146142	372.159105	5.637862
5.339317	378.282498	5.642867
5.575128	373.246790	5.647872
5.438704	371.986879	5.652877
5.402374	364.601977	5.657882
5.028376	368.112343	5.662886
5.154011	383.582713	5.667891
5.166997	379.309593	5.672896
5.174747	378.438387	5.677901
5.132535	396.526226	5.682906
5.596983	399.667943	5.687910
5.596889	406.346820	5.692915
5.685356	411.974093	5.697920
5.618488	409.330186	5.702925
5.608874	399.277153	5.707930
5.501823	396.247231	5.712934
5.866329	394.073585	5.717939
5.689076	404.212954	5.722944
5.528347	399.941736	5.727949
5.530926	403.415253	5.732954
5.516331	407.394507	5.737958
5.668932	397.208489	5.742963
5.536325	402.664750	5.747968
5.838042	399.906145	5.752973
5.694891	398.175878	5.757978
5.861213	401.674360	5.762982
5.730750	395.129948	5.767987
5.713619	402.896681	5.772992
5.801823	406.265031	5.777997
5.862054	411.387354	5.783002
6.179419	408.607314	5.788006
6.146161	406.429549	5.793011
5.790450	405.064786	5.798016
5.934393	398.913985	5.803021
5.933167	400.360094	5.808026
5.826124	405.024561	5.813030
5.896351	391.440863	5.818035
5.857724	402.786069	5.823040
6.275876	405.346572	5.828045
5.870706	406.938232	5.833050
5.906845	404.126323	5.838054
6.290430	402.993745	5.843059
5.870626	411.576560	5.848064
6.012389	401.003089	5.853069
5.877212	399.818912	5.858074
5.945551	407.360279	5.863078
6.205549	397.005571	5.868083
6.089888	409.482840	5.873088
6.337524	403.932734	5.878093
6.051760	401.902103	5.883098
5.847177	411.653445	5.888102
6.196079	396.134120	5.893107
5.623710	411.043152	5.898112
5.994430	409.077342	5.903117
5.984847	403.032853	5.908122
5.986553	415.751170	5.913126
6.143063	405.029851	5.918131
6.055007	413.703059	5.923136
6.821944	406.701656	5.928141
6.123426	409.582656	5.933146
5.957159	403.961357	5.938150
6.254786	404.028677	5.943155
6.115057	410.878133	5.948160
6.539042	410.555489	5.953165
6.539604	405.426916	5.958170
6.448082	404.966739	5.963174
6.444360	400.908207	5.968179
5.803748	408.146195	5.973184
6.202548	406.356324	5.978189
6.039472	415.345014	5.983194
6.497644	425.046307	5.988198
6.383477	425.965938	5.993203
6.382035	419.489889	5.998208
6.399674	414.263722	6.003213
6.350281	411.797414	6.008218
6.225383	412.759856	6.013222
6.304940	410.289163	6.018227
6.534704	426.347544	6.023232
6.427809	420.005078	6.028237
6.436487	414.280434	6.033242
5.890688	413.745898	6.038246
6.488968	419.973515	6.043251
6.381761	429.893112	6.048256
6.843346	421.629725	6.053261
6.202415	407.654394	6.058266
6.410549	401.642234	6.063270
6.272868	391.327691	6.068275
6.445616	409.176215	6.073280
6.759812	401.812307	6.078285
6.300330	394.645555	6.083290
6.224429	405.569489	6.088294
6.400637	396.148579	6.093299
6.379123	412.252646	6.098304
6.496016	404.511518	6.103309
6.346680	404.440058	6.108314
6.061368	399.577744	6.113318
5.952396	404.672792	6.118323
6.260358	409.560143	6.123328
6.310454	417.389116	6.128333
6.405102	428.004762	6.133338
6.395018	435.599558	6.138342
6.620839	419.488881	6.143347
6.232210	417.556624	6.148352
6.530223	408.499444	6.153357
6.499463	397.468943	6.158362
6.347973	406.848126	6.163366
6.457310	403.509047	6.168371
6.379985	409.140149	6.173376
6.340369	404.043182	6.178381
6.272102	395.628703	6.183386
6.195772	402.699182	6.188390
6.265555	400.498945	6.193395
6.416895	412.326931	6.198400
6.068807	404.924418	6.203405
6.576396	417.107884	6.208410
6.449563	418.725538	6.213414
6.304002	407.893355	6.218419
6.161132	408.599179	6.223424
6.130088	422.129405	6.228429
6.360330	428.019212	6.233434
6.178310	429.057045	6.238438
6.742274	421.881789	6.243443
6.830992	435.146482	6.248448
6.528099	418.963618	6.253453
6.353806	409.474229	6.258458
6.011775	404.953001	6.263462
6.162851	407.242133	6.268467
6.319665	422.258391	6.273472
6.321727	423.125008	6.278477
6.714785	427.467510	6.283482
6.241049	427.389929	6.288486
6.385821	411.013542	6.293491
5.976866	413.747932	6.298496
6.411993	425.199261	6.303501
6.521419	427.893562	6.308506
6.510199	433.261208	6.313510
6.592658	419.419304	6.318515
6.282418	411.719787	6.323520
6.121880	403.209029	6.328525
6.225316	403.316266	6.333530
6.532539	427.246733	6.338534
6.566707	417.022311	6.343539
6.137949	414.381320	6.348544
6.291828	409.994367	6.353549
6.221492	413.643828	6.358554
6.493802	420.435057	6.363558
6.363423	415.222591	6.368563
6.377306	417.080794	6.373568
6.351852	425.212678	6.378573
6.598283	423.788371	6.383578
6.708772	427.997973	6.388582
6.484574	413.359382	6.393587
6.198501	425.012297	6.398592
6.120389	406.301138	6.403597
6.361958	410.101049	6.408602
6.192648	409.494869	6.413606
6.273793	407.919287	6.418611
6.366431	412.916308	6.423616
6.605726	408.411566	6.428621
6.433833	407.831102	6.433626
6.640855	408.111938	6.438630
6.766731	407.465836	6.443635
6.671325	409.632233	6.448640
6.383736	408.038493	6.453645
6.220191	407.896491	6.458650
6.190672	416.234656	6.463654
6.299936	412.398869	6.468659
6.102062	415.157135	6.473664
6.284502	407.408900	6.478669
6.583722	409.646346	6.483674
6.398595	409.615295	6.488678
6.498432	406.641543	6.493683
6.425804	402.451435	6.498688
6.380240	406.464016	6.503693
6.289612	404.431284	6.508698
6.412341	413.077794	6.513702
6.500676	401.405359	6.518707
6.647411	409.377378	6.523712
6.542791	407.909997	6.528717
6.619309	413.232253	6.533722
6.777147	407.351359	6.538726
6.527928	398.845006	6.543731
6.443504	404.752471	6.548736
6.233974	381.771800	6.553741
6.468352	385.601306	6.558746
5.948226	388.128481	6.563750
6.304458	396.077161	6.568755
6.365485	408.390702	6.573760
6.551356	405.134545	6.578765
6.587888	402.819294	6.583770
6.486045	394.941597	6.588774
6.333782	384.660981	6.593779
6.262413	383.308617	6.598784
6.345204	382.938190	6.603789
6.213033	388.593699	6.608794
6.568669	402.019029	6.613798
6.636432	400.002611	6.618803
6.232135	381.212870	6.623808
6.137904	382.316039	6.628813
6.082461	382.739240	6.633818
6.363725	404.395802	6.638822
6.403644	391.022501	6.643827
6.541884	401.419326	6.648832
6.687903	398.615512	6.653837
6.276838	390.362316	6.658842
6.438519	386.432898	6.663846
6.087385	387.266267	6.668851
6.205606	396.359572	6.673856
6.487361	407.610290	6.678861
6.891163	399.245234	6.683866
6.394197	396.146689	6.688870
6.717103	385.285412	6.693875
6.308990	392.331939	6.698880
6.118037	388.318565	6.703885
6.355126	383.940726	6.708890
6.219512	390.270666	6.713894
6.703208	386.407855	6.718899
6.114953	392.172790	6.723904
5.756705	390.099732	6.728909
6.142638	396.480837	6.733914
6.316968	406.666362	6.738918
6.280094	419.004741	6.743923
6.139172	418.384622	6.748928
6.574494	421.306275	6.753933
6.457338	409.140838	6.758938
5.995355	422.400056	6.763942
6.414144	409.122407	6.768947
6.484825	417.334140	6.773952
6.594826	410.739391	6.778957
6.491317	414.761052	6.783962
6.520853	417.442558	6.788966
6.401586	400.288123	6.793971
5.944276	397.563022	6.798976
6.369205	403.919036	6.803981
6.598218	413.766961	6.808986
6.523911	409.507511	6.813990
6.431135	390.137430	6.818995
5.886439	389.109168	6.824000
6.200683	404.780964	6.829005
6.505121	406.862565	6.834010
6.111568	409.638835	6.839014
6.513992	409.597984	6.844019
6.549821	413.616797	6.849024
6.449872	415.445378	6.854029
6.294115	402.514023	6.859034
6.289209	420.529601	6.864038
6.576796	403.836609	6.869043
6.349606	408.678093	6.874048
6.320375	403.373851	6.879053
6.510297	396.513480	6.884058
6.048864	400.319131	6.889062
6.174850	400.951191	6.894067
6.257823	413.925698	6.899072
6.549483	405.578210	6.904077
6.663785	413.514182	6.909082
6.642103	409.176883	6.914086
6.362932	389.674652	6.919091
5.690945	390.264059	6.924096
6.126296	401.266077	6.929101
6.295976	402.758176	6.934106
6.312084	405.736018	6.939110
6.404118	409.584669	6.944115
6.591398	406.081515	6.949120
6.156358	413.220856	6.954125
6.770299	409.761584	6.959130
6.189136	420.192041	6.964134
6.256750	415.046632	6.969139
6.516193	410.301446	6.974144
6.430703	406.989729	6.979149
6.221295	414.394280	6.984154
6.313185	421.530159	6.989158
6.220108	416.254899	6.994163
6.234217	411.234935	6.999168
6.326863	419.000294	7.004173
6.541896	406.899872	7.009178
6.136481	422.048514	7.014182
6.403449	406.535689	7.019187
6.264188	411.591191	7.024192
6.127290	417.060784	7.029197
6.627763	414.558942	7.034202
6.257671	419.679088	7.039206
6.550944	411.103549	7.044211
6.365029	420.788696	7.049216
6.442195	414.961569	7.054221
6.530356	414.346687	7.059226
6.279621	414.870091	7.064230
6.717157	408.439163	7.069235
6.504094	417.369246	7.074240
6.626969	404.732761	7.079245
6.300375	395.254588	7.084250
6.034022	398.741766	7.089254
6.499233	398.861924	7.094259
6.160825	407.014361	7.099264
6.071907	405.202828	7.104269
6.411425	417.235454	7.109274
5.939235	417.281019	7.114278
6.126181	420.656048	7.119283
6.344370	416.379242	7.124288
6.663570	420.211285	7.129293
6.605934	410.883955	7.134298
6.339874	414.212900	7.139302
6.180831	416.636046	7.144307
6.210048	421.026062	7.149312
6.586425	417.388871	7.154317
6.328438	405.640979	7.159322
6.349643	413.847808	7.164326
6.401858	412.083765	7.169331
6.465463	420.524403	7.174336
6.305177	414.294711	7.179341
6.343613	414.383658	7.184346
6.205942	422.042733	7.189350
6.551883	415.018702	7.194355
6.411324	418.384932	7.199360
6.317920	417.833299	7.204365
6.670312	414.614327	7.209370
6.731536	412.396448	7.214374
6.279018	411.224026	7.219379
6.268255	407.751901	7.224384
6.008317	419.400717	7.229389
6.347231	408.650815	7.234394
6.109366	412.351836	7.239398
6.066372	421.293240	7.244403
6.330917	414.911561	7.249408
6.409557	411.918982	7.254413
6.394226	413.300863	7.259418
6.020813	412.426100	7.264422
6.155564	410.307434	7.269427
6.169230	416.667778	7.274432
6.237208	407.368226	7.279437
6.450352	412.969637	7.284442
6.405859	418.481700	7.289446
6.565490	406.016629	7.294451
6.413225	418.872970	7.299456
6.268113	416.352055	7.304461
6.653658	418.155189	7.309466
6.179485	401.815675	7.314470
6.338532	411.510044	7.319475
6.269993	418.205977	7.324480
6.362683	420.099290	7.329485
6.545857	414.954757	7.334490
6.175245	412.117991	7.339494
6.492392	405.060509	7.344499
6.685303	409.573574	7.349504
6.144045	421.162064	7.354509
6.674044	415.298788	7.359514
6.547198	418.656542	7.364518
6.578198	417.769036	7.369523
6.198838	424.931296	7.374528
6.153794	422.334588	7.379533
6.420754	410.482297	7.384538
6.119348	417.243190	7.389542
6.427823	415.321935	7.394547
6.085336	415.568645	7.399552
6.346216	417.802608	7.404557
6.871360	413.939624	7.409562
6.641663	415.225376	7.414566
6.439761	403.335818	7.419571
6.306805	408.203665	7.424576
6.467890	412.107938	7.429581
6.803969	405.101275	7.434586
6.301759	404.781377	7.439590
6.387594	393.609221	7.444595
5.953063	402.301909	7.449600
6.325611	409.105902	7.454605
6.526084	407.277501	7.459610
6.186902	417.192307	7.464614
6.452360	405.985672	7.469619
6.445474	420.464419	7.474624
6.302859	405.882655	7.479629
6.393749	404.093570	7.484634
6.343470	409.182587	7.489638
6.416185	408.402443	7.494643
6.198623	414.337098	7.499648
6.362911	428.757393	7.504653
6.333750	414.100898	7.509658
6.378226	426.315802	7.514662
6.053047	417.865635	7.519667
6.668898	421.723966	7.524672
6.371420	422.128142	7.529677
6.486855	412.590193	7.534682
6.306563	424.523932	7.539686
6.485806	409.891736	7.544691
6.631437	409.789878	7.549696
6.169228	402.294513	7.554701
6.586293	395.892108	7.559706
5.998249	404.877774	7.564710
6.256815	406.169282	7.569715
6.361980	406.032635	7.574720
6.379021	418.710585	7.579725
6.442883	414.429485	7.584730
6.398592	416.325277	7.589734
6.318872	411.968596	7.594739
6.488663	409.170548	7.599744
6.099897	409.870606	7.604749
6.527993	410.749567	7.609754
6.232943	422.150781	7.614758
6.478846	415.996654	7.619763
6.331514	416.845549	7.624768
6.128912	422.205213	7.629773
6.189359	413.615532	7.634778
6.040484	425.262770	7.639782
6.068245	408.360542	7.644787
6.271278	413.618682	7.649792
6.169041	415.953832	7.654797
6.094537	414.016651	7.659802
6.263362	415.936000	7.664806
6.333334	417.855019	7.669811
6.365325	419.055476	7.674816
6.229383	418.757285	7.679821
6.488086	413.350978	7.684826
6.172120	418.601850	7.689830
5.675709	411.826863	7.694835
6.542504	418.660989	7.699840
6.134671	416.583042	7.704845
6.568714	411.566886	7.709850
6.625885	419.382096	7.714854
6.232192	415.368843	7.719859
6.089467	422.639561	7.724864
5.846371	422.453074	7.729869
6.831187	429.509163	7.734874
6.258445	436.590993	7.739878
6.338966	439.903606	7.744883
6.530142	438.032365	7.749888
6.473950	436.956035	7.754893
6.613968	430.945046	7.759898
6.268034	418.378841	7.764902
6.609532	416.597947	7.769907
6.442340	414.112130	7.774912
6.413537	419.947609	7.779917
6.659602	417.539413	7.784922
6.414784	424.221839	7.789926
6.332934	417.271161	7.794931
6.797465	419.394120	7.799936
6.592805	422.229382	7.804941
6.546751	411.587254	7.809946
5.981359	422.606876	7.814950
6.516791	414.230680	7.819955
6.268363	413.140178	7.824960
6.230503	418.667021	7.829965
6.251463	407.872024	7.834970
6.246620	417.408573	7.839974
6.406424	409.094397	7.844979
6.068634	412.798419	7.849984
6.195199	416.129123	7.854989
6.629983	408.774793	7.859994
6.445336	417.422008	7.864998
6.416829	414.310172	7.870003
6.356911	415.974291	7.875008
6.345881	417.320695	7.880013
6.438592	407.821111	7.885018
6.356478	410.393557	7.890022
6.473525	412.624745	7.895027
6.511640	411.856349	7.900032
6.455008	416.158573	7.905037
6.602492	418.777306	7.910042
6.483570	416.568669	7.915046
6.671972	414.463743	7.920051
6.741468	412.836200	7.925056
6.476908	405.667377	7.930061
6.471140	392.421459	7.935066
6.041496	389.625584	7.940070
6.423678	397.940364	7.945075
6.455798	397.808834	7.950080
6.354264	385.887743	7.955085
6.260126	383.377829	7.960090
6.193220	389.162319	7.965094
6.402255	399.554378	7.970099
6.509094	406.137405	7.975104
6.235783	406.832029	7.980109
6.465110	415.408053	7.985114
6.376466	415.833293	7.990118
6.346136	411.168642	7.995136
6.293365	393.501661	8.000154
6.233512	410.081890	8.005171
6.460562	408.992353	8.010189
6.676799	414.146569	8.015206
6.211504	390.633520	8.020224
6.696954	384.441693	8.025242
6.129415	384.880959	8.030259
6.575190	382.832522	8.035277
5.882371	383.433425	8.040294
6.369986	400.470653	8.045312
6.707127	406.098218	8.050330
6.634080	404.197340	8.055347
6.214347	392.542741	8.060365
6.258076	404.928537	8.065382
6.401821	408.500460	8.070400
6.422849	417.147112	8.075418
6.324767	412.974864	8.080435
6.682278	405.850041	8.085453
6.563296	415.272851	8.090470
6.212358	414.302276	8.095488
6.404350	419.018488	8.100506
6.303118	417.727927	8.105523
6.571048	413.286897	8.110541
6.560508	413.711473	8.115558
6.341761	410.296576	8.120576
6.565410	405.752034	8.125594
6.392420	410.171987	8.130611
6.584227	406.711698	8.135629
6.261999	412.417331	8.140646
6.153750	409.348031	8.145664
6.550229	408.680063	8.150682
6.441522	414.860317	8.155699
6.411747	407.392239	8.160717
6.572007	413.612399	8.165734
6.228368	409.368175	8.170752
6.310806	406.294244	8.175770
6.234484	415.432666	8.180787
6.423936	411.982212	8.185805
6.273164	414.053968	8.190822
6.626085	421.238003	8.195840
6.566674	424.541964	8.200858
6.798795	433.180796	8.205875
6.663555	417.006758	8.210893
6.363451	429.739928	8.215910
6.441400	417.483480	8.220928
6.733816	421.757933	8.225946
6.666038	430.472153	8.230963
6.935365	417.472522	8.235981
6.235273	418.301779	8.240998
6.348367	420.149160	8.246016
6.534941	423.736465	8.251034
6.830084	442.214509	8.256051
6.896558	433.895066	8.261069
6.444917	434.991504	8.266086
6.325865	436.436610	8.271104
6.593567	439.503132	8.276122
6.738392	450.317337	8.281139
7.281750	436.845574	8.286157
6.776113	430.774304	8.291174
6.394790	419.426087	8.296192
6.798363	418.671802	8.301210
6.400953	427.532341	8.306227
6.501687	432.092445	8.311245
6.569811	435.641509	8.316262
6.823033	439.253088	8.321280
6.837411	443.896152	8.326298
6.940849	451.381216	8.331315
6.997408	434.902560	8.336333
6.557028	426.722495	8.341350
6.570663	423.877088	8.346368
6.529787	426.004209	8.351386
6.756243	440.204355	8.356403
6.770063	440.192777	8.361421
6.632751	437.137494	8.366438
6.748331	440.849533	8.371456
7.106408	441.140617	8.376474
6.578072	441.583209	8.381491
6.833196	441.817841	8.386509
7.102201	451.681644	8.391526
6.637631	436.972963	8.396544
6.829739	424.578706	8.401562
6.176624	429.095981	8.406579
6.443882	438.177425	8.411597
6.721028	445.644737	8.416614
6.389543	443.796970	8.421632
6.876982	442.600362	8.426650
6.741199	446.743099	8.431667
6.650589	432.752144	8.436685
6.837771	443.244133	8.441702
7.013318	435.557684	8.446720
7.091234	432.768475	8.451738
6.765494	439.727498	8.456755
6.938456	436.355361	8.461773
6.636545	445.652218	8.466790
6.726878	443.665777	8.471808
7.019161	433.894023	8.476826
7.239722	432.322673	8.481843
7.161551	427.853817	8.486861
6.858714	440.495906	8.491878
6.877230	444.125327	8.496896
7.405706	429.652373	8.501914
7.111678	439.418197	8.506931
6.919277	440.568689	8.511949
7.046794	429.806603	8.516966
6.449351	421.685862	8.521984
6.678258	423.931656	8.527002
6.864141	433.603349	8.532019
6.795863	441.181584	8.537037
6.581137	442.329262	8.542054
6.840912	425.784061	8.547072
6.767854	440.359333	8.552090
6.666797	447.475656	8.557107
6.677030	441.392981	8.562125
6.933252	432.381102	8.567143
6.660866	434.759088	8.572160
6.746368	433.035333	8.577178
6.931648	451.177155	8.582195
6.992772	455.052362	8.587213
7.322831	458.393135	8.592231
7.206466	460.446882	8.597248
7.176399	445.868928	8.602266
7.552167	441.546692	8.607283
6.768171	437.762770	8.612301
7.158783	444.344472	8.617319
7.060243	439.162451	8.622336
6.972800	431.015446	8.627354
6.945476	437.018857	8.632371
7.017403	433.817183	8.637389
6.916823	431.434630	8.642407
7.028106	437.971735	8.647424
6.660175	433.595615	8.652442
7.161661	437.635346	8.657459
6.839488	440.879497	8.662477
7.177152	428.582349	8.667495
6.775350	437.894853	8.672512
7.253283	451.225644	8.677530
7.156133	449.031897	8.682547
7.129403	456.196537	8.687565
7.041666	437.102280	8.692583
6.963473	447.203513	8.697600
7.151067	451.317675	8.702618
7.144292	453.183840	8.707635
7.135912	461.680490	8.712653
7.388570	457.020939	8.717671
7.249456	451.371908	8.722688
7.290504	444.123088	8.727706
7.276834	437.772765	8.732723
7.210835	433.529215	8.737741
7.326863	439.977217	8.742759
7.135444	441.512556	8.747776
7.125252	435.044926	8.752794
7.115616	434.087144	8.757811
6.964986	439.933154	8.762829
7.229239	429.389481	8.767847
7.229305	435.735732	8.772864
7.110459	433.990346	8.777882
7.159039	434.538202	8.782899
7.271828	430.799960	8.787917
7.252076	431.913933	8.792935
7.350670	445.455632	8.797952
7.404816	437.008734	8.802970
7.281272	433.976539	8.807987
7.054186	434.204676	8.813005
7.379471	438.335130	8.818023
7.259081	434.122192	8.823040
7.367819	428.017776	8.828058
7.003835	439.034768	8.833075
7.256885	438.932061	8.838093
7.431781	434.470889	8.843111
6.859759	441.736739	8.848128
7.376092	440.226341	8.853146
7.535317	445.957533	8.858163
7.427870	436.797509	8.863181
7.581699	435.798336	8.868199
7.415999	442.299948	8.873216
7.301157	429.556157	8.878234
7.145625	443.712017	8.883251
7.185001	437.028340	8.888269
7.436705	426.799054	8.893287
6.955921	437.039098	8.898304
7.513555	441.379296	8.903322
7.287004	443.955225	8.908339
7.177897	443.884015	8.913357
7.693640	454.239326	8.918375
7.583575	447.108854	8.923392
7.349093	433.285605	8.928410
7.399028	443.729672	8.933427
7.275015	442.275423	8.938445
7.379785	427.013651	8.943463
7.107436	441.708511	8.948480
7.525330	444.574780	8.953498
7.448001	455.086129	8.958515
7.551153	455.451869	8.963533
7.683821	442.082319	8.968551
7.171015	443.295635	8.973568
7.133334	446.296400	8.978586
7.704483	447.538693	8.983603
7.248196	465.613797	8.988621
7.468672	452.249416	8.993639
7.499436	458.303692	8.998656
7.582213	455.194986	9.003674
7.799684	454.463547	9.008691
7.534550	456.221873	9.013709
7.456217	433.487567	9.018727
7.179876	439.927619	9.023744
7.641993	453.055766	9.028762
7.832832	452.391615	9.033779
7.463883	450.262544	9.038797
7.261531	445.888879	9.043815
7.306551	450.350421	9.048832
7.419721	452.686934	9.053850
7.613886	460.965659	9.058867
7.763277	463.930804	9.063885
7.720700	463.050765	9.068903
7.424532	452.310868	9.073920
7.685334	448.669350	9.078938
7.861090	460.864089	9.083955
7.275895	447.042132	9.088973
7.475565	455.206384	9.093991
7.479131	460.747380	9.099008
7.668042	458.597171	9.104026
7.884378	456.717217	9.109043
7.542482	455.177187	9.114061
7.725533	446.372423	9.119079
7.523379	447.584402	9.124096
7.551160	453.623365	9.129114
7.545219	457.240842	9.134131
7.590326	460.032981	9.139149
7.749059	453.501008	9.144167
7.351145	457.811049	9.149184
7.399987	454.417332	9.154202
7.781038	456.620357	9.159219
7.484787	459.507005	9.164237
7.459695	455.705157	9.169255
7.284348	460.775576	9.174272
7.676266	451.073407	9.179290
7.402510	457.042854	9.184307
7.259748	456.339455	9.189325
7.377351	456.434692	9.194343
7.496281	470.752693	9.199360
7.545969	475.920399	9.204378
7.951973	482.272490	9.209395
7.949218	488.492972	9.214413
8.257373	479.027971	9.219431
8.154566	473.619394	9.224448
7.618115	459.306959	9.229466
7.872694	459.992950	9.234483
7.487276	458.112606	9.239501
8.065047	457.649757	9.244519
7.702320	462.304575	9.249536
7.682529	467.555747	9.254554
7.747564	460.404146	9.259571
7.687667	463.398927	9.264589
8.023293	453.686643	9.269607
7.836940	455.129673	9.274624
7.992637	452.318806	9.279642
7.697969	459.089935	9.284659
7.749640	470.335306	9.289677
7.821022	460.102696	9.294695
7.697903	466.263135	9.299712
7.259062	465.044402	9.304730
7.898347	475.512910	9.309747
8.035159	482.055499	9.314765
8.165591	486.191248	9.319783
7.900204	471.148379	9.324800
7.497711	470.514076	9.329818
8.143946	483.108477	9.334835
8.037004	489.174872	9.339853
8.237612	471.963567	9.344871
7.465333	466.319065	9.349888
7.693551	465.674302	9.354906
8.028958	474.132871	9.359923
7.998127	484.797896	9.364941
8.335487	478.455674	9.369959
8.134764	465.053138	9.374976
7.806340	461.567054	9.379994
8.072358	454.118882	9.385011
7.559307	457.102614	9.390029
7.747020	470.592499	9.395047
7.887473	489.296796	9.400064
8.076975	476.776681	9.405082
8.257478	475.845909	9.410099
8.152857	478.765651	9.415117
7.936759	465.775771	9.420135
8.215048	460.279085	9.425152
8.005322	457.190963	9.430170
8.563752	459.732263	9.435187
8.175522	464.327962	9.440205
7.817970	455.642609	9.445223
8.097364	458.189760	9.450240
8.199995	467.076110	9.455258
8.139491	461.455784	9.460275
7.761285	461.174277	9.465293
7.907096	463.821252	9.470311
8.305600	457.829213	9.475328
7.805008	455.121174	9.480346
8.194465	458.888134	9.485363
7.729442	455.764275	9.490381
7.753405	470.292813	9.495399
8.084891	472.920165	9.500416
8.254835	488.618719	9.505434
8.628343	487.111761	9.510451
8.298978	479.734774	9.515469
7.979247	462.920581	9.520487
8.246455	466.126039	9.525504
7.722281	466.571134	9.530522
8.191911	469.590245	9.535539
8.043312	480.560893	9.540557
8.453243	478.634825	9.545575
8.586653	477.026633	9.550592
7.786258	470.780629	9.555610
8.493574	465.264057	9.560627
7.932591	465.613936	9.565645
7.766563	476.404279	9.570663
8.224631	476.269448	9.575680
8.533582	488.714731	9.580698
8.519970	485.453868	9.585715
8.089351	487.657840	9.590733
8.355387	481.241587	9.595751
7.914567	474.150304	9.600768
8.158996	485.523271	9.605786
8.359000	483.620627	9.610803
8.329164	488.024480	9.615821
7.883923	486.355476	9.620839
8.313526	487.601015	9.625856
8.141784	495.290156	9.630874
8.366368	493.153289	9.635891
8.046115	486.355531	9.640909
7.983006	486.586378	9.645927
8.086933	489.463978	9.650944
8.025438	491.805773	9.655962
8.243116	477.416191	9.660979
8.206721	491.092681	9.665997
7.786361	486.453367	9.671015
8.218020	494.054277	9.676032
8.386885	507.853252	9.681050
8.839553	505.276710	9.686067
8.357975	495.518878	9.691085
8.275975	496.781461	9.696103
8.547974	489.550085	9.701120
8.529154	496.278007	9.706138
8.632577	490.335346	9.711155
8.179600	492.814218	9.716173
8.151088	491.793119	9.721191
8.426165	485.883525	9.726208
8.476381	501.319987	9.731226
8.638064	499.571666	9.736243
8.429675	496.372876	9.741261
8.443641	490.302223	9.746279
8.384581	482.860792	9.751296
8.297450	500.155424	9.756314
8.510362	508.330249	9.761331
8.634279	513.959700	9.766349
8.731254	509.589612	9.771367
8.853504	487.997751	9.776384
8.181924	498.450758	9.781402
8.241839	499.189341	9.786419
8.542399	492.950708	9.791437
8.480394	508.493121	9.796455
8.887292	491.268410	9.801472
8.491460	495.896866	9.806490
8.301391	487.040091	9.811507
8.298790	499.786656	9.816525
8.443249	508.985206	9.821543
8.642126	512.113017	9.826560
8.589251	507.258331	9.831578
8.907881	512.525918	9.836595
8.517152	509.513484	9.841613
8.408676	511.597558	9.846631
8.848671	517.272159	9.851648
8.694072	518.662882	9.856666
8.826178	506.416823	9.861683
8.604553	492.727211	9.866701
8.317803	492.207315	9.871719
8.600733	504.776605	9.876736
8.561734	509.131407	9.881754
8.754726	499.460381	9.886771
8.725103	505.148599	9.891789
8.797622	504.395689	9.896807
8.953360	507.700669	9.901824
8.333240	502.616130	9.906842
8.688014	500.973252	9.911859
8.729931	508.651013	9.916877
8.640394	513.237794	9.921895
9.035476	504.904701	9.926912
8.701222	514.354981	9.931930
8.677750	516.712912	9.936947
8.780436	514.595142	9.941965
8.504429	515.234881	9.946983
8.768984	510.286278	9.952000
8.701349	508.245687	9.957018
8.672317	509.118125	9.962035
8.926729	510.141810	9.967053
8.600522	511.190197	9.972071
8.695395	511.664530	9.977088
8.808855	515.559952	9.982106
8.888037	506.821924	9.987123
9.017892	508.480498	9.992141
8.757121	515.609249	9.997159
8.815044	513.495337	10.002176
8.917536	510.910545	10.007194
8.783379	513.506721	10.012211
8.744338	516.876934	10.017229
8.640914	522.743977	10.022247
8.684635	516.132173	10.027264
8.712611	519.002744	10.032282
9.168918	510.644276	10.037299
8.668683	508.071871	10.042317
8.614070	508.616963	10.047335
8.912835	502.337583	10.052352
8.779486	515.281368	10.057370
8.740423	508.439544	10.062387
8.488064	508.788404	10.067405
8.498082	512.109905	10.072423
9.109147	510.013466	10.077440
8.844361	515.773247	10.082458
8.766501	520.080493	10.087475
8.965426	516.918865	10.092493
9.162573	528.207750	10.097511
9.361100	531.184143	10.102528
9.038899	521.871533	10.107546
9.167563	520.996218	10.112563
9.216203	518.861669	10.117581
8.646907	514.895769	10.122599
9.028326	505.898951	10.127616
8.781260	512.539567	10.132634
8.997198	515.090357	10.137651
8.907247	517.941535	10.142669
9.049578	540.154799	10.147687
9.319881	528.840113	10.152704
9.080429	519.183184	10.157722
8.948069	520.321117	10.162739
8.860253	516.125146	10.167757
9.064514	526.220038	10.172775
9.302813	540.456278	10.177792
9.300187	537.442989	10.182810
9.060044	522.759033	10.187827
9.239497	524.996809	10.192845
9.112597	519.061825	10.197863
8.717777	523.159961	10.202880
8.814776	523.015432	10.207898
9.120310	542.296671	10.212915
9.707077	551.198725	10.217933
9.342373	542.495515	10.222951
9.217327	530.501167	10.227968
8.905550	521.704469	10.232986
9.309052	531.998517	10.238003
9.144319	532.930088	10.243021
9.421214	541.334741	10.248039
9.558142	525.856410	10.253056
9.347728	525.210944	10.258074
9.139067	519.137293	10.263091
8.861299	515.819984	10.268109
8.799225	522.311700	10.273127
9.460196	537.062372	10.278144
9.316702	539.956657	10.283162
9.179628	537.917475	10.288179
9.374485	537.978517	10.293197
9.370650	543.366065	10.298215
9.601529	535.052374	10.303232
9.278393	519.702935	10.308250
8.994934	518.153744	10.313267
9.210438	522.213057	10.318285
9.220656	531.117075	10.323303
9.251594	540.241909	10.328320
9.373714	537.713998	10.333338
9.390439	541.722410	10.338355
9.189468	541.419443	10.343373
9.230110	548.870206	10.348391
9.309572	545.127696	10.353408
9.354188	547.408691	10.358426
9.368065	537.241851	10.363443
9.479414	538.095452	10.368461
9.313723	541.583342	10.373479
9.681680	543.062604	10.378496
9.733795	541.028492	10.383514
9.588740	537.643049	10.388531
9.500949	543.438222	10.393549
9.093311	539.626867	10.398567
9.196629	537.313337	10.403584
9.407145	536.822823	10.408602
9.387975	539.763899	10.413619
9.565142	543.157046	10.418637
9.058357	551.334202	10.423655
9.392485	541.631572	10.428672
9.502264	540.497287	10.433690
9.261181	544.142155	10.438707
9.731820	542.803008	10.443725
9.423804	531.825082	10.448743
9.340288	535.906003	10.453760
9.574118	537.500952	10.458778
9.415035	536.320431	10.463795
9.418019	533.624996	10.468813
9.214143	533.148917	10.473831
9.356815	526.051397	10.478848
9.459423	530.926809	10.483866
9.246810	557.541194	10.488883
9.749750	552.703550	10.493901
9.518237	557.934274	10.498919
9.489822	559.494575	10.503936
9.519499	557.255697	10.508954
9.685683	557.403282	10.513971
9.600099	560.279029	10.518989
9.710742	564.039204	10.524007
9.973826	553.063301	10.529024
9.801810	551.468244	10.534042
9.169108	559.579928	10.539059
9.536524	553.166699	10.544077
9.668237	566.917892	10.549095
9.741870	559.023299	10.554112
9.748813	552.470892	10.559130
9.774895	562.760978	10.564147
9.937857	561.662539	10.569165
9.642363	563.457189	10.574183
9.516440	554.924841	10.579200
9.498916	553.933576	10.584218
9.406657	559.047808	10.589235
9.753957	565.734171	10.594253
9.631495	557.330666	10.599271
9.585866	562.125172	10.604288
9.754692	554.212510	10.609306
9.637075	554.278331	10.614323
10.030005	551.749011	10.619341
9.755555	555.039353	10.624359
9.854953	554.585183	10.629376
10.139113	557.219963	10.634394
9.764673	558.373738	10.639411
10.055271	558.388222	10.644429
9.790598	558.578068	10.649447
9.537219	568.867762	10.654464
10.090939	554.772601	10.659482
9.904827	562.353571	10.664499
9.969387	558.502940	10.669517
9.356217	563.657766	10.674535
9.263807	558.818728	10.679552
9.773924	577.872293	10.684570
9.943195	579.325884	10.689587
10.201315	584.688180	10.694605
10.000406	590.668347	10.699623
10.435809	579.895800	10.704640
10.386031	572.478124	10.709658
9.952229	566.083131	10.714675
9.979263	558.874329	10.719693
9.962257	569.666625	10.724711
9.616347	568.240822	10.729728
10.043517	568.164481	10.734746
10.057764	564.309109	10.739763
10.123805	559.634590	10.744781
10.014139	574.351406	10.749799
10.012171	571.091858	10.754816
9.700315	562.023756	10.759834
9.783998	565.223273	10.764851
10.026356	582.879766	10.769869
10.053694	587.454565	10.774887
9.884198	583.381828	10.779904
10.171637	580.102180	10.784922
10.209854	587.916253	10.789939
10.139763	579.889537	10.794957
10.149168	586.786638	10.799975
10.226459	594.222211	10.804992
10.600482	587.845804	10.810010
9.865909	585.824495	10.815027
9.764976	583.290500	10.820045
9.776286	585.734507	10.825063
10.068003	581.804100	10.830080
10.095897	589.326304	10.835098
10.179657	596.218071	10.840115
9.997176	589.057863	10.845133
9.999138	591.184603	10.850151
10.017114	586.921547	10.855168
10.261942	584.683669	10.860186
9.859597	599.768251	10.865203
10.232723	590.696951	10.870221
10.512724	591.183306	10.875239
10.284979	596.568083	10.880256
10.287605	587.539056	10.885274
10.215859	597.349033	10.890291
10.542541	587.372993	10.895309
10.562110	590.178621	10.900327
10.327579	587.984291	10.905344
10.463861	587.685286	10.910362
10.310511	596.188934	10.915379
10.307016	592.778145	10.920397
10.429664	584.708604	10.925415
10.297841	588.617227	10.930432
10.728532	587.697742	10.935450
10.456387	586.377144	10.940467
10.409734	588.946997	10.945485
10.526538	590.427744	10.950503
10.265633	589.061204	10.955520
10.656340	592.048521	10.960538
10.301044	596.787414	10.965555
10.338321	589.816835	10.970573
10.405734	593.508051	10.975591
10.737136	591.398617	10.980608
10.573799	587.186060	10.985626
10.029367	590.316740	10.990643
10.208846	589.515510	10.995661
10.612720	585.823146	11.000679
10.519629	594.311041	11.005696
10.380685	589.813797	11.010714
10.350039	587.716909	11.015731
10.550061	578.947289	11.020749
10.409517	586.622115	11.025767
10.577961	592.506543	11.030784
10.870609	584.151593	11.035802
10.524444	586.010989	11.040819
10.555927	590.629320	11.045837
10.592529	584.154305	11.050855
10.374166	587.653613	11.055872
10.416292	585.513766	11.060890
10.091200	588.600611	11.065907
10.662905	593.020693	11.070925
10.504994	592.483762	11.075943
10.365757	612.715225	11.080960
10.754264	603.865569	11.085978
10.962045	615.256984	11.090995
10.608117	613.841900	11.096013
10.750155	597.545360	11.101031
10.101781	599.388992	11.106048
10.503936	603.195018	11.111066
10.470140	609.963199	11.116083
10.882537	613.584589	11.121101
10.739110	608.437953	11.126119
10.863100	623.963947	11.131136
10.756420	614.974123	11.136154
10.714669	614.150751	11.141171
11.103578	620.521349	11.146189
11.136863	619.825073	11.151207
10.832064	613.731740	11.156224
10.707710	592.872662	11.161242
10.707693	597.890403	11.166259
10.743826	594.274590	11.171277
10.827025	606.562825	11.176295
10.647217	609.440720	11.181312
10.365937	616.774694	11.186330
10.594547	605.523296	11.191347
10.504954	610.220563	11.196365
10.917681	608.694827	11.201383
10.961045	624.590057	11.206400
11.139410	614.479451	11.211418
10.745945	605.818586	11.216435
10.721839	616.709852	11.221453
10.534792	615.262310	11.226471
10.588344	611.422860	11.231488
11.067403	607.349486	11.236506
10.858547	614.908796	11.241523
10.509036	612.350629	11.246541
11.055057	615.152670	11.251559
10.681107	610.408222	11.256576
10.814499	606.063963	11.261594
11.040741	619.633130	11.266611
11.433825	626.842514	11.271629
11.459574	614.512060	11.276647
10.814613	618.927119	11.281664
11.169530	613.374199	11.286682
10.905001	613.485128	11.291699
10.716049	613.069824	11.296717
11.000631	617.856788	11.301735
10.918991	618.185213	11.306752
11.145223	622.801441	11.311770
11.396792	611.357096	11.316787
11.276813	610.804754	11.321805
11.305016	610.017758	11.326823
11.262984	621.079091	11.331840
11.424555	615.285067	11.336858
11.156467	613.966987	11.341875
11.029570	612.510021	11.346893
11.271526	614.308829	11.351911
10.954334	610.779930	11.356928
11.272483	618.297694	11.361946
11.411289	618.509529	11.366963
10.989852	620.068300	11.371981
11.323775	608.645766	11.376999
10.933095	616.634349	11.382016
11.228352	604.132288	11.387034
11.280054	611.041707	11.392051
11.100730	610.173618	11.397069
11.458276	603.850279	11.402087
11.351627	613.173433	11.407104
11.147499	617.472084	11.412122
11.417576	609.606649	11.417139
11.299572	613.222780	11.422157
11.125770	618.829484	11.427175
11.423924	619.761116	11.432192
11.191028	613.438768	11.437210
11.298583	609.704465	11.442227
11.005332	616.835190	11.447245
11.143127	606.888734	11.452263
10.964826	616.794311	11.457280
11.083887	614.191129	11.462298
10.911778	625.812484	11.467315
11.131333	631.177681	11.472333
11.456006	634.408879	11.477351
11.396604	647.306460	11.482368
11.649490	644.123732	11.487386
11.604275	639.971550	11.492403
11.403963	639.416015	11.497421
11.678693	637.627877	11.502439
11.503842	641.912480	11.507456
11.371479	641.557736	11.512474
12.207711	640.394829	11.517491
11.848836	625.792507	11.522509
12.019963	625.030453	11.527527
11.692974	621.651409	11.532544
11.213853	611.665911	11.537562
11.664519	615.028842	11.542579
11.500401	611.308703	11.547597
11.454856	613.370306	11.552615
11.270036	617.296706	11.557632
11.597348	618.242704	11.562650
11.803540	606.108044	11.567667
11.532583	620.569305	11.572685
11.868413	604.479078	11.577703
11.573624	607.848354	11.582720
11.449333	607.587020	11.587738
11.600609	611.059975	11.592755
11.562147	609.854238	11.597773
11.867249	607.786792	11.602791
11.553953	616.763631	11.607808
11.366804	612.740990	11.612826
11.379855	608.500791	11.617843
11.384284	624.067610	11.622861
11.612187	624.060359	11.627879
11.818449	639.134823	11.632896
11.761846	645.152359	11.637914
11.946697	627.839232	11.642931
11.781596	643.391604	11.647949
11.799852	630.235498	11.652967
11.732461	624.284842	11.657984
11.371254	624.818015	11.663002
12.158406	638.274066	11.668019
11.871180	641.471752	11.673037
11.680759	626.688403	11.678055
12.215493	629.422788	11.683072
11.808791	627.362725	11.688090
11.503425	611.931528	11.693107
11.768246	629.748648	11.698125
11.851387	639.161998	11.703143
11.509587	639.979306	11.708160
11.986403	649.798036	11.713178
11.774865	633.661002	11.718195
11.861765	644.102550	11.723213
11.700185	635.092916	11.728231
11.565348	648.873313	11.733248
11.497453	636.879406	11.738266
12.065181	636.869404	11.743283
11.842202	642.972967	11.748301
11.454874	636.993541	11.753319
11.391753	635.962078	11.758336
11.880474	649.319730	11.763354
12.251383	654.304616	11.768371
12.275325	667.167062	11.773389
12.155583	654.174571	11.778407
11.672203	649.500907	11.783424
11.882950	644.920457	11.788442
12.391737	642.931546	11.793459
11.749366	651.347740	11.798477
12.069723	653.812763	11.803495
12.352230	658.480143	11.808512
12.037164	652.833370	11.813530
12.258123	634.454235	11.818547
11.715885	643.870899	11.823565
12.216029	647.630025	11.828583
12.380190	659.306012	11.833600
12.245782	650.219529	11.838618
12.411278	639.356693	11.843635
12.383870	643.176385	11.848653
11.970275	647.422657	11.853671
12.612635	638.523742	11.858688
11.917452	648.724916	11.863706
12.223968	633.576523	11.868723
11.775031	645.477949	11.873741
11.770967	639.574171	11.878759
12.405940	649.721567	11.883776
12.458090	654.668035	11.888794
12.248981	656.534365	11.893811
12.427564	667.996660	11.898829
12.226183	658.680827	11.903847
12.397229	663.211039	11.908864
12.108398	662.353794	11.913882
12.456992	660.904373	11.918899
12.276658	672.094705	11.923917
12.309640	676.280481	11.928935
12.469356	656.036380	11.933952
12.460921	663.573776	11.938970
12.367601	655.853620	11.943987
12.148327	655.828072	11.949005
12.338064	655.025232	11.954023
11.988728	655.742737	11.959040
12.299394	668.617064	11.964058
12.572703	660.059983	11.969075
12.544374	661.020680	11.974093
12.153922	666.412037	11.979111
12.528067	662.575994	11.984128
12.199022	666.938410	11.989146
12.279080	668.844641	11.994163
12.308876	666.795077	11.999181
12.497424	669.009356	12.004199
12.399632	655.704157	12.009216
12.302886	661.671184	12.014234
12.292938	665.611221	12.019251
12.328216	656.870531	12.024269
12.269523	671.554193	12.029287
12.496112	687.212490	12.034304
12.437598	697.478038	12.039322
12.491130	689.832688	12.044339
12.548677	696.807496	12.049357
12.545356	690.269270	12.054375
12.781933	693.429076	12.059392
12.558708	694.682242	12.064410
12.555401	690.895865	12.069427
12.604718	693.176143	12.074445
12.525420	689.032445	12.079463
12.608377	692.617106	12.084480
12.722819	701.817302	12.089498
12.860439	687.096113	12.094515
12.874109	700.417782	12.099533
12.917763	695.437468	12.104551
13.091758	687.874230	12.109568
12.976240	699.764477	12.114586
13.123456	694.695353	12.119603
12.788601	678.839531	12.124621
12.565461	667.103456	12.129639
12.794187	672.505098	12.134656
12.744101	683.649782	12.139674
12.633988	683.020154	12.144691
12.294613	695.863807	12.149709
12.932273	698.077149	12.154727
12.859809	697.785602	12.159744
12.685388	697.790896	12.164762
12.609499	690.033280	12.169779
12.850577	694.874418	12.174797
12.639332	690.328518	12.179815
12.902266	692.051464	12.184832
12.645933	695.850231	12.189850
12.977602	695.776229	12.194867
12.628071	697.737149	12.199885
12.540973	697.230145	12.204903
12.946708	706.062813	12.209920
12.998214	704.394850	12.214938
13.351814	715.798196	12.219955
13.118944	696.385576	12.224973
13.030837	692.767119	12.229991
13.234525	686.070228	12.235008
12.760915	693.043050	12.240026
12.934813	692.510932	12.245043
13.158167	697.547351	12.250061
13.181649	701.715687	12.255079
12.926922	690.549433	12.260096
13.135005	705.402762	12.265114
13.083701	710.649475	12.270131
13.532638	716.196508	12.275149
13.148502	697.202062	12.280167
13.106421	694.472638	12.285184
12.980638	694.202069	12.290202
13.247762	703.356252	12.295219
13.208708	700.342332	12.300237
13.196588	700.934420	12.305255
13.505442	693.933872	12.310272
13.032691	693.206428	12.315290
13.132588	697.738328	12.320307
13.451841	697.928203	12.325325
13.319149	699.296573	12.330343
12.997618	692.047658	12.335360
12.822064	714.187868	12.340378
13.181574	714.412461	12.345395
13.410831	710.207790	12.350413
13.141696	719.310305	12.355431
13.469373	720.600234	12.360448
13.344570	723.923963	12.365466
13.494081	727.299388	12.370483
13.278098	721.545551	12.375501
13.191423	722.326045	12.380519
13.311720	707.424518	12.385536
13.083116	717.937633	12.390554
13.097696	714.912151	12.395571
13.304508	716.284133	12.400589
13.408125	715.939751	12.405607
13.657850	711.394202	12.410624
13.451227	718.539796	12.415642
13.760055	710.523079	12.420659
13.570792	713.503458	12.425677
13.273717	724.431247	12.430695
13.555777	721.449061	12.435712
13.284282	719.247883	12.440730
13.522714	715.922241	12.445747
13.555585	713.704933	12.450765
13.554562	712.398649	12.455783
13.444358	713.233323	12.460800
13.686100	716.748929	12.465818
13.485915	714.224154	12.470835
13.285026	711.185096	12.475853
13.077114	719.201892	12.480871
13.868989	721.514151	12.485888
13.634101	739.040447	12.490906
13.958152	744.165243	12.495923
13.910046	729.129137	12.500941
13.697235	726.429615	12.505959
13.827474	714.505597	12.510976
13.459406	720.635075	12.515994
13.836242	715.268037	12.521011
13.866188	714.414492	12.526029
13.813056	715.625230	12.531047
13.673005	711.626745	12.536064
13.424176	721.139488	12.541082
13.772002	713.328098	12.546099
13.510155	715.972712	12.551117
13.688326	729.117150	12.556135
14.055214	734.459294	12.561152
14.270226	742.293071	12.566170
13.723791	729.326355	12.571187
13.759336	713.854278	12.576205
13.686649	719.135902	12.581223
13.878253	734.686113	12.586240
14.172449	742.901959	12.591258
13.694948	745.687664	12.596275
13.953890	750.484993	12.601293
13.800679	749.303537	12.606311
13.894113	749.670805	12.611328
13.740442	752.614055	12.616346
14.183359	736.658410	12.621363
14.438583	733.510014	12.626381
13.952868	749.731249	12.631399
14.205422	745.084263	12.636416
14.008146	742.508536	12.641434
13.994662	737.496138	12.646451
14.065148	743.162435	12.651469
13.845738	747.892700	12.656487
13.781351	737.002707	12.661504
13.927890	739.056320	12.666522
14.068727	732.858408	12.671539
14.486623	731.691613	12.676557
13.980413	744.463611	12.681575
13.789712	747.112861	12.686592
14.234287	743.653930	12.691610
13.970999	747.043543	12.696627
14.157268	742.709900	12.701645
13.879074	747.922747	12.706663
14.085905	743.488052	12.711680
14.000921	746.868663	12.716698
13.609352	742.309977	12.721715
14.045216	748.793185	12.726733
13.963209	756.474690	12.731751
14.271157	766.884832	12.736768
13.835150	765.738217	12.741786
14.129708	772.587556	12.746803
14.091672	763.050416	12.751821
14.002418	770.698349	12.756839
14.151569	768.598515	12.761856
14.361704	775.716703	12.766874
14.077194	778.390123	12.771891
14.175732	769.831971	12.776909
14.003702	772.528793	12.781927
14.244929	781.775437	12.786944
14.374266	787.896432	12.791962
14.450580	792.589842	12.796979
14.656036	800.308377	12.801997
14.554208	803.830494	12.807015
14.440592	789.479945	12.812032
14.479581	787.419460	12.817050
14.180380	785.503482	12.822067
14.832281	790.015190	12.827085
14.549836	799.454346	12.832103
14.321811	784.449539	12.837120
14.477150	789.203151	12.842138
14.487909	795.102885	12.847155
14.659901	796.035359	12.852173
14.542567	791.897597	12.857191
14.495731	792.908538	12.862208
14.816242	795.928979	12.867226
14.623151	795.665798	12.872243
14.849092	791.259656	12.877261
14.460772	791.737121	12.882279
14.459862	793.409898	12.887296
14.619359	793.053603	12.892314
14.419455	799.365043	12.897331
14.602718	802.328094	12.902349
14.745937	803.116753	12.907367
15.045951	803.546330	12.912384
14.811359	811.930266	12.917402
14.808939	804.445113	12.922419
14.938801	798.832723	12.927437
14.876971	801.414453	12.932455
14.755227	797.977970	12.937472
14.940742	797.718585	12.942490
14.521942	793.776379	12.947507
14.969717	787.978482	12.952525
14.900264	795.550740	12.957543
14.668196	798.032909	12.962560
15.115321	791.613419	12.967578
14.948524	799.869962	12.972595
15.141795	797.772679	12.977613
14.815394	795.984038	12.982631
14.716468	786.226051	12.987648
14.775906	789.631379	12.992666
14.431771	799.168564	12.997683
14.895155	788.006499	13.002701
14.533012	804.713352	13.007719
14.966405	800.331509	13.012736
15.085784	791.328267	13.017754
14.722594	801.370213	13.022771
15.075961	806.837573	13.027789
15.125477	798.037779	13.032807
14.590206	795.000605	13.037824
15.191092	805.611025	13.042842
15.056452	808.948935	13.047859
15.101202	801.778285	13.052877
15.187764	810.761999	13.057895
14.988832	815.129311	13.062912
15.326449	810.219672	13.067930
15.181218	824.484672	13.072947
15.518711	812.130484	13.077965
14.879090	811.609061	13.082983
14.860249	808.121739	13.088000
15.088123	816.300673	13.093018
15.162129	822.193663	13.098035
15.358231	813.579178	13.103053
15.284840	819.839244	13.108071
15.287842	827.791484	13.113088
15.517014	821.623883	13.118106
14.889926	820.393594	13.123123
15.313810	817.938283	13.128141
15.711257	816.010980	13.133159
15.575428	820.018111	13.138176
15.757520	811.648819	13.143194
15.338662	804.828519	13.148211
15.224988	787.173846	13.153229
14.868223	805.732318	13.158247
15.438752	815.735272	13.163264
15.783007	811.225381	13.168282
15.457555	819.503635	13.173299
15.466682	819.050979	13.178317
15.378781	818.007609	13.183335
15.385238	823.324201	13.188352
15.928392	809.880594	13.193370
15.590638	809.002604	13.198387
15.587867	804.143143	13.203405
15.459405	803.244984	13.208423
15.153568	810.964739	13.213440
15.638825	804.561360	13.218458
15.276739	821.580645	13.223475
15.339133	809.247471	13.228493
15.771678	817.034575	13.233511
15.385800	822.879699	13.238528
15.908437	813.507149	13.243546
15.516101	816.885437	13.248563
15.670773	816.350016	13.253581
15.540862	815.786601	13.258599
15.491541	817.706807	13.263616
15.834631	811.467712	13.268634
15.936453	819.417089	13.273651
15.890311	814.125762	13.278669
16.030368	815.258901	13.283687
15.713169	820.490503	13.288704
15.777088	814.080552	13.293722
15.481228	819.365615	13.298739
15.491269	813.453257	13.303757
15.326898	812.797411	13.308775
15.204523	813.185870	13.313792
15.799166	820.048171	13.318810
15.847686	839.306884	13.323827
15.849524	836.340183	13.328845
15.718463	840.854658	13.333863
15.600213	835.555687	13.338880
16.056159	837.352549	13.343898
16.042991	846.235141	13.348915
15.775636	842.584778	13.353933
16.021290	835.717154	13.358951
15.923565	846.844158	13.363968
16.195483	851.547962	13.368986
15.898607	845.402814	13.374003
16.026192	841.996686	13.379021
15.962356	846.453292	13.384039
16.350354	843.555474	13.389056
16.105398	840.829413	13.394074
16.132280	846.745573	13.399091
16.119750	847.303016	13.404109
15.849895	838.180855	13.409127
15.666695	849.756756	13.414144
15.936489	841.828147	13.419162
15.881381	849.982007	13.424179
15.956172	844.261467	13.429197
16.390355	847.709077	13.434215
15.855854	851.882821	13.439232
16.470960	845.386499	13.444250
16.301792	846.416610	13.449267
15.888929	849.608771	13.454285
16.152759	853.180903	13.459303
16.329544	870.598645	13.464320
16.418593	859.438382	13.469338
16.427496	872.041399	13.474355
16.547237	868.084226	13.479373
16.426700	863.085409	13.484391
16.442519	848.395795	13.489408
16.409953	839.239610	13.494426
16.355801	836.934936	13.499443
16.107639	838.270915	13.504461
16.476236	854.733933	13.509479
16.114898	868.543676	13.514496
16.454011	871.542280	13.519514
16.747800	860.709702	13.524531
16.310644	868.686743	13.529549
16.693020	865.710907	13.534567
16.531846	875.323608	13.539584
16.604402	868.946998	13.544602
16.368797	877.217514	13.549619
16.615351	863.422704	13.554637
16.500472	871.466017	13.559655
16.701043	870.156538	13.564672
16.719427	863.583290	13.569690
16.578911	866.492939	13.574707
16.524726	860.407592	13.579725
17.019182	858.474552	13.584743
16.590720	873.847481	13.589760
16.783285	861.841016	13.594778
16.815123	868.314987	13.599795
16.735084	859.879446	13.604813
16.626128	843.899720	13.609831
16.470883	853.618778	13.614848
17.059197	856.480504	13.619866
16.963927	864.192536	13.624883
16.650269	855.714705	13.629901
16.641370	852.213194	13.634919
16.508518	859.025392	13.639936
16.562933	859.231517	13.644954
16.654204	867.132075	13.649971
16.614729	855.556449	13.654989
16.771752	853.953991	13.660007
16.540939	857.127097	13.665024
16.802647	853.835652	13.670042
16.762003	866.392779	13.675059
16.444575	858.190095	13.680077
16.441785	862.769685	13.685095
16.911302	880.801138	13.690112
16.944759	880.190033	13.695130
16.901551	880.354649	13.700147
16.974469	886.714893	13.705165
17.411901	887.940300	13.710183
17.189887	899.793716	13.715200
17.088122	890.796671	13.720218
17.254089	892.673687	13.725235
16.921537	890.573572	13.730253
17.215682	881.593397	13.735271
17.058663	885.247254	13.740288
17.294652	881.688433	13.745306
17.219120	886.459308	13.750323
17.273365	895.766867	13.755341
17.614296	877.400244	13.760359
17.370717	888.581685	13.765376
17.365084	873.848073	13.770394
17.212450	866.380118	13.775411
17.161520	865.536081	13.780429
17.150393	874.610873	13.785447
16.945140	876.019028	13.790464
17.333479	885.905400	13.795482
17.123696	881.630622	13.800499
17.156923	882.120936	13.805517
17.351785	878.341340	13.810535
17.267208	881.333746	13.815552
17.565989	877.399012	13.820570
17.267170	887.314154	13.825587
17.411030	890.245523	13.830605
17.361556	879.438314	13.835623
17.173757	885.678459	13.840640
17.229032	882.028031	13.845658
17.536380	882.967704	13.850675
17.748250	890.041485	13.855693
17.992719	882.558642	13.860711
17.394563	880.708429	13.865728
17.248750	884.811813	13.870746
17.659105	875.024476	13.875763
17.452656	877.540512	13.880781
17.629393	876.039106	13.885799
17.333683	892.129714	13.890816
17.499283	884.700253	13.895834
17.631560	887.721800	13.900851
17.527621	879.438319	13.905869
17.733604	879.699592	13.910887
17.786785	880.022677	13.915904
17.772997	892.070682	13.920922
17.842402	885.372666	13.925939
17.619136	884.132750	13.930957
17.695138	880.264478	13.935975
17.616824	891.883933	13.940992
17.745486	876.494957	13.946010
17.918329	878.935786	13.951027
17.817101	886.172232	13.956045
17.837278	879.431438	13.961063
17.629660	892.832104	13.966080
17.930618	906.765327	13.971098
17.834492	911.914980	13.976115
18.260261	913.180086	13.981133
18.198621	902.560963	13.986151
17.951243	886.085331	13.991168
17.833090	883.582394	13.996186
18.030979	886.783010	14.001203
17.957574	885.592197	14.006221
17.877307	886.800887	14.011239
18.043994	903.690064	14.016256
18.132476	905.418274	14.021274
18.121395	902.434651	14.026291
18.087097	906.359621	14.031309
18.078690	902.728634	14.036327
18.285403	912.854919	14.041344
18.444026	907.414716	14.046362
18.241139	890.199956	14.051379
17.832306	882.333476	14.056397
18.117018	886.880650	14.061415
18.501917	893.823179	14.066432
17.714268	887.855898	14.071450
18.175519	897.639334	14.076467
17.904668	910.163132	14.081485
18.244020	897.947451	14.086503
18.069620	910.292034	14.091520
18.237480	904.537958	14.096538
18.184470	897.597183	14.101555
18.355135	912.301912	14.106573
17.947915	914.884125	14.111591
18.191934	910.437251	14.116608
17.863712	910.356188	14.121626
18.041814	903.136201	14.126643
18.300960	929.330083	14.131661
18.483174	922.431340	14.136679
18.342113	932.839346	14.141696
18.609917	941.289794	14.146714
18.595582	927.722006	14.151731
18.605890	936.020291	14.156749
18.586454	926.884095	14.161767
18.819210	924.881598	14.166784
18.464378	914.560872	14.171802
18.056176	911.200808	14.176819
18.623567	926.004337	14.181837
18.949706	923.551703	14.186855
18.862219	928.943007	14.191872
18.624792	929.526222	14.196890
19.040775	900.585242	14.201907
18.256377	907.767789	14.206925
18.835238	913.307150	14.211943
18.534748	925.920811	14.216960
18.690904	929.475115	14.221978
18.886146	919.809821	14.226995
18.593701	935.136244	14.232013
18.796262	928.994867	14.237031
18.748954	927.102522	14.242048
18.498366	930.720556	14.247066
18.850948	929.652346	14.252083
18.643731	933.061611	14.257101
18.886810	924.941490	14.262119
18.775622	927.095466	14.267136
18.857727	922.774945	14.272154
18.989571	930.937419	14.277171
18.490242	930.990464	14.282189
18.793899	930.769371	14.287207
18.539020	934.634233	14.292224
18.418646	932.513493	14.297242
19.184742	938.140291	14.302259
19.196971	953.920772	14.307277
19.020720	944.326294	14.312295
19.085099	934.220744	14.317312
19.083904	948.002523	14.322330
19.334778	939.464603	14.327347
19.256050	939.729461	14.332365
18.980031	934.808634	14.337383
19.181076	926.786617	14.342400
18.995751	932.136446	14.347418
19.310306	938.323147	14.352435
19.149587	942.962216	14.357453
19.463528	945.248402	14.362471
19.737901	940.566390	14.367488
19.161898	936.064953	14.372506
19.090906	930.045331	14.377523
19.112624	930.266048	14.382541
19.501028	930.202092	14.387559
19.476987	929.208671	14.392576
19.204500	935.171766	14.397594
19.331878	927.694627	14.402611
19.375437	932.307999	14.407629
19.274357	941.381139	14.412647
19.622624	940.398812	14.417664
19.438745	943.069113	14.422682
19.827135	938.760560	14.427699
19.349711	936.664204	14.432717
19.525263	934.332994	14.437735
19.362941	923.802217	14.442752
19.284233	935.352335	14.447770
19.667971	937.570779	14.452787
19.128380	944.856996	14.457805
19.142590	952.400432	14.462823
19.423617	945.732353	14.467840
19.420101	947.276164	14.472858
19.500669	948.809957	14.477875
19.430228	951.730731	14.482893
19.670715	948.796048	14.487911
19.803818	946.963798	14.492928
19.423978	952.041149	14.497946
19.816789	946.157139	14.502963
19.598985	952.149541	14.507981
19.623079	950.608929	14.512999
19.857304	944.386845	14.518016
19.597587	956.217803	14.523034
19.832859	955.808607	14.528051
19.542006	972.005823	14.533069
19.757572	972.549623	14.538087
20.157723	971.000581	14.543104
19.717339	975.588802	14.548122
19.808490	975.612446	14.553139
19.969053	981.892718	14.558157
20.048463	978.904372	14.563175
20.344041	976.895182	14.568192
20.060397	983.803637	14.573210
20.229103	974.009926	14.578227
20.025834	963.539191	14.583245
19.875192	958.491415	14.588263
20.048412	958.688395	14.593280
20.016901	974.343201	14.598298
20.141001	970.432660	14.603315
20.214161	967.552594	14.608333
19.780894	970.511284	14.613351
20.457418	959.574497	14.618368
20.294382	964.999739	14.623386
20.330759	972.653322	14.628403
20.439084	971.661250	14.633421
20.218680	966.826375	14.638439
20.205366	965.960661	14.643456
20.126347	973.430350	14.648474
20.155765	975.770587	14.653491
20.026729	975.159691	14.658509
20.185935	980.736423	14.663527
20.555965	967.853160	14.668544
20.135799	978.582637	14.673562
20.316908	980.308965	14.678579
20.146087	978.868318	14.683597
20.464357	971.859875	14.688615
20.495003	969.608169	14.693632
20.239258	977.553679	14.698650
20.272109	978.369107	14.703667
20.204864	980.667684	14.708685
20.250025	977.590029	14.713703
20.574579	971.902899	14.718720
20.299143	986.109533	14.723738
20.497330	988.079342	14.728755
20.816027	996.029531	14.733773
20.841431	989.092214	14.738791
20.668553	984.928395	14.743808
20.692030	988.894824	14.748826
20.716483	987.704451	14.753843
20.566156	1001.042572	14.758861
20.692082	999.249312	14.763879
20.794521	1000.202162	14.768896
20.710129	999.401232	14.773914
20.782739	991.424556	14.778931
20.975549	991.116688	14.783949
20.803776	994.356307	14.788967
21.103562	994.618665	14.793984
20.649745	979.702720	14.799002
20.877400	997.308278	14.804019
21.177482	992.918873	14.809037
20.730763	990.300140	14.814055
21.065672	988.262696	14.819072
20.914426	986.986241	14.824090
20.906971	988.716867	14.829107
21.208728	987.814409	14.834125
20.799592	983.747569	14.839143
21.195545	973.934032	14.844160
20.830268	983.638730	14.849178
21.129204	981.329209	14.854195
20.974057	982.726365	14.859213
20.977021	987.122046	14.864231
20.781333	985.417048	14.869248
20.988896	987.439037	14.874266
20.928128	988.319627	14.879283
21.440786	985.689437	14.884301
20.934536	989.956617	14.889319
21.186102	984.738517	14.894336
20.969827	982.970472	14.899354
21.300150	977.497034	14.904371
21.188866	985.183224	14.909389
20.961743	988.658736	14.914407
21.344867	987.409010	14.919424
21.113249	987.694667	14.924442
21.056660	992.610928	14.929459
21.526457	997.072326	14.934477
21.153921	1011.679207	14.939495
21.484693	1001.036412	14.944512
21.422973	1004.463920	14.949530
21.432390	1006.636879	14.954547
21.463061	1003.053398	14.959565
21.482555	1008.790886	14.964583
21.593046	1004.535326	14.969600
21.685513	1014.963596	14.974618
21.520931	1017.495183	14.979635
21.382143	1010.747688	14.984653
21.022134	1016.967523	14.989671
21.497786	1011.212524	14.994688
21.461934	1014.610735	14.999706
21.374399	1008.985004	15.004723
21.528394	1008.105697	15.009741
21.467583	1002.021339	15.014759
21.520085	1017.808189	15.019776
21.904079	1031.488655	15.024794
21.816177	1032.578628	15.029811
22.112601	1034.867571	15.034829
21.878169	1025.181178	15.039847
21.838791	1002.512628	15.044864
21.731153	1018.075257	15.049882
21.347562	1024.879466	15.054899
22.037440	1029.978586	15.059917
21.934161	1036.609490	15.064935
22.071117	1031.560814	15.069952
21.798027	1034.235639	15.074970
21.806956	1034.180646	15.079987
22.210006	1034.748722	15.085005
21.743873	1029.075004	15.090023
22.172657	1029.029969	15.095040
21.908775	1031.876922	15.100058
22.011926	1031.832413	15.105075
22.230123	1030.965136	15.110093
22.199777	1033.393641	15.115111
22.062150	1024.534694	15.120128
21.814467	1025.965286	15.125146
22.020378	1025.096779	15.130163
22.455079	1022.406214	15.135181
21.942852	1038.836994	15.140199
22.393533	1028.970671	15.145216
22.184864	1026.516609	15.150234
22.010105	1034.872340	15.155251
22.072608	1023.820277	15.160269
22.190489	1030.425995	15.165287
22.415685	1038.637010	15.170304
22.030235	1049.796597	15.175322
22.315116	1051.667622	15.180339
22.692943	1048.200156	15.185357
22.630595	1056.727635	15.190375
22.433056	1050.386967	15.195392
22.493609	1041.739961	15.200410
22.668281	1045.660623	15.205427
22.923122	1041.376126	15.210445
22.280873	1034.306710	15.215463
22.571817	1020.208175	15.220480
22.436584	1021.517005	15.225498
22.442857	1040.021994	15.230515
23.089423	1043.079755	15.235533
22.442181	1047.706717	15.240551
22.579668	1045.015377	15.245568
22.595292	1053.363378	15.250586
22.893411	1051.410587	15.255603
23.115102	1054.667466	15.260621
22.660844	1037.419364	15.265639
22.742620	1032.477165	15.270656
22.488626	1029.648347	15.275674
22.963165	1044.289794	15.280691
22.882984	1041.689366	15.285709
22.773482	1045.809188	15.290727
22.746649	1046.766516	15.295744
23.005445	1048.887784	15.300762
22.690809	1047.687418	15.305779
22.908615	1047.602854	15.310797
22.878309	1042.687681	15.315815
23.172147	1048.227561	15.320832
23.120673	1050.391130	15.325850
22.887657	1054.962660	15.330867
22.636554	1051.480123	15.335885
22.411919	1056.599459	15.340903
22.790209	1050.708221	15.345920
23.116078	1042.186906	15.350938
22.963756	1051.605807	15.355955
23.072714	1066.872606	15.360973
23.244201	1077.376896	15.365991
23.388029	1072.475457	15.371008
23.198362	1083.080517	15.376026
23.308299	1076.092052	15.381043
23.377079	1076.415852	15.386061
23.326526	1073.533061	15.391079
23.355561	1073.863088	15.396096
23.544182	1066.767622	15.401114
23.345002	1074.391882	15.406131
23.560261	1066.367576	15.411149
23.486976	1058.735627	15.416167
23.146856	1054.228760	15.421184
23.065753	1056.463245	15.426202
23.234031	1065.267024	15.431219
23.372312	1067.826905	15.436237
23.329603	1078.314262	15.441255
23.515246	1066.277186	15.446272
23.968391	1063.028294	15.451290
23.584684	1064.073096	15.456307
23.673794	1066.473422	15.461325
23.561213	1067.134911	15.466343
23.677753	1068.947105	15.471360
23.416845	1064.131174	15.476378
23.679882	1066.747250	15.481395
23.749867	1058.894034	15.486413
23.385627	1068.226224	15.491431
23.445066	1063.943935	15.496448
23.661844	1072.541299	15.501466
23.576032	1070.304672	15.506483
23.979476	1074.151625	15.511501
24.062010	1077.524987	15.516519
24.014581	1073.306778	15.521536
23.972152	1064.432895	15.526554
23.935516	1074.524815	15.531571
23.528069	1062.366069	15.536589
23.384032	1074.658670	15.541607
23.985402	1084.142540	15.546624
24.187145	1084.136233	15.551642
24.036953	1088.439170	15.556659
24.295190	1085.700503	15.561677
23.983862	1077.452579	15.566695
24.072266	1091.734836	15.571712
24.159112	1073.448848	15.576730
24.174798	1086.376007	15.581747
24.601761	1081.007319	15.586765
24.457056	1085.233654	15.591783
24.177873	1081.496730	15.596800
24.281885	1074.607025	15.601818
24.273831	1084.372576	15.606835
24.171604	1082.274221	15.611853
24.581326	1084.892563	15.616871
24.381531	1085.198483	15.621888
24.360159	1081.001435	15.626906
24.419265	1093.625146	15.631923
24.131140	1090.893185	15.636941
24.564757	1090.380325	15.641959
24.181482	1090.557199	15.646976
24.089908	1087.024414	15.651994
24.230176	1094.371431	15.657011
24.455919	1081.621149	15.662029
24.177428	1092.312716	15.667047
24.296541	1085.988696	15.672064
24.460899	1081.052480	15.677082
24.324858	1081.840725	15.682099
24.880029	1090.994159	15.687117
24.989891	1089.711501	15.692135
24.634206	1083.424003	15.697152
24.839684	1086.418335	15.702170
24.804370	1098.141643	15.707187
25.133765	1083.853992	15.712205
24.763866	1092.533819	15.717223
24.485255	1092.353461	15.722240
24.786043	1092.546235	15.727258
24.562929	1087.566582	15.732275
24.522390	1099.483217	15.737293
25.051145	1099.289972	15.742311
24.782686	1108.291590	15.747328
24.755224	1115.421894	15.752346
24.589886	1117.537039	15.757363
24.743612	1107.799252	15.762381
24.881623	1111.328033	15.767399
24.865683	1114.429647	15.772416
25.150271	1108.777139	15.777434
24.853379	1112.465581	15.782451
24.952033	1110.521945	15.787469
24.855661	1114.447218	15.792487
24.867761	1132.408581	15.797504
25.539675	1131.154624	15.802522
25.307745	1142.523750	15.807539
25.173771	1136.182561	15.812557
25.231193	1127.602277	15.817575
25.287073	1135.139262	15.822592
25.501215	1132.132936	15.827610
25.288566	1132.930030	15.832627
25.615456	1129.211747	15.837645
25.421513	1103.067428	15.842663
25.422275	1111.439876	15.847680
25.429179	1109.665253	15.852698
25.207343	1117.299392	15.857715
25.256939	1120.737885	15.862733
25.761160	1120.046701	15.867751
25.634155	1128.827346	15.872768
25.551887	1127.407527	15.877786
25.603253	1137.776035	15.882803
25.581529	1130.224341	15.887821
25.763280	1120.419038	15.892839
25.478761	1123.291330	15.897856
25.819121	1125.538686	15.902874
25.973419	1126.836875	15.907891
25.963310	1112.081678	15.912909
25.872587	1104.493467	15.917927
25.413971	1105.562632	15.922944
25.722070	1100.752215	15.927962
25.528750	1106.052854	15.932979
25.620834	1115.326196	15.937997
25.834408	1125.849166	15.943015
25.505020	1124.657418	15.948032
25.811076	1119.231922	15.953050
26.160110	1122.935929	15.958067
25.781684	1130.073891	15.963085
26.133475	1124.205717	15.968103
25.973360	1127.197376	15.973120
26.229596	1123.764725	15.978138
25.926315	1129.757956	15.983155
25.796284	1133.906263	15.988173
25.907657	1119.346624	15.993191
25.557922	1122.737229	15.998208
25.765903	1130.556500	16.003226
26.003258	1135.183742	16.008243
26.268047	1150.969008	16.013261
26.342873	1153.093866	16.018279
26.198756	1159.131598	16.023296
26.550674	1163.052917	16.028314
26.423318	1161.637004	16.033331
26.430195	1157.138860	16.038349
26.616590	1154.073761	16.043367
26.391650	1153.168610	16.048384
26.431098	1133.955848	16.053402
26.174894	1141.093599	16.058419
26.080354	1147.123559	16.063437
26.295384	1153.026121	16.068455
26.356010	1162.395936	16.073472
26.686083	1146.972014	16.078490
26.522213	1152.346950	16.083507
26.843520	1151.678112	16.088525
26.815387	1150.959880	16.093543
26.411567	1157.603203	16.098560
26.640017	1157.819935	16.103578
26.716867	1158.675815	16.108595
26.493189	1149.691430	16.113613
27.071130	1145.368908	16.118631
26.941132	1152.228108	16.123648
26.979881	1157.063203	16.128666
26.831136	1153.981184	16.133683
26.740594	1150.303054	16.138701
26.878914	1152.790357	16.143719
26.836755	1156.621937	16.148736
26.689706	1151.002330	16.153754
26.768397	1161.423376	16.158771
26.596048	1162.813773	16.163789
26.946686	1153.269176	16.168807
26.601409	1154.790811	16.173824
26.896680	1150.853411	16.178842
26.940265	1160.759238	16.183859
27.082320	1169.024366	16.188877
27.413889	1172.835265	16.193895
27.398553	1176.438580	16.198912
27.123864	1162.422243	16.203930
27.040926	1160.844733	16.208947
26.758910	1174.519204	16.213965
27.131727	1175.533845	16.218983
27.134435	1172.320793	16.224000
27.623968	1179.862437	16.229018
27.597338	1166.309017	16.234035
27.411727	1170.077867	16.239053
27.652394	1167.016886	16.244071
27.267204	1172.934600	16.249088
27.355935	1177.591451	16.254106
27.417485	1182.337772	16.259123
27.268640	1172.830397	16.264141
27.400158	1171.613769	16.269159
27.337809	1177.364135	16.274176
27.337369	1177.455779	16.279194
27.291316	1175.613706	16.284211
27.164068	1167.785033	16.289229
27.666363	1171.809029	16.294247
27.329225	1178.205221	16.299264
27.549948	1186.398069	16.304282
27.665738	1192.492922	16.309299
27.372349	1191.945640	16.314317
28.380149	1187.530512	16.319335
27.966766	1191.069960	16.324352
28.090804	1185.584598	16.329370
28.096219	1176.103546	16.334387
27.868392	1167.507974	16.339405
27.958766	1159.477946	16.344423
27.975612	1172.436544	16.349440
27.876842	1164.060600	16.354458
28.035153	1161.182940	16.359475
28.009925	1171.320466	16.364493
28.089256	1172.343220	16.369511
27.877226	1180.231476	16.374528
27.973660	1191.918423	16.379546
27.901211	1190.730595	16.384563
28.028783	1197.407442	16.389581
28.013681	1194.771547	16.394599
27.722785	1194.580489	16.399616
28.274352	1191.303530	16.404634
28.102223	1186.268523	16.409651
28.283173	1197.086988	16.414669
28.146678	1195.571516	16.419687
28.315095	1196.842251	16.424704
27.832097	1202.645908	16.429722
28.013364	1193.386609	16.434739
28.190845	1208.365076	16.439757
28.740024	1221.619010	16.444775
28.784305	1220.090991	16.449792
28.512229	1214.948556	16.454810
28.947506	1214.126156	16.459827
28.461064	1219.977697	16.464845
28.789595	1209.142621	16.469863
28.882959	1217.996083	16.474880
28.582354	1202.816099	16.479898
28.901006	1187.166708	16.484915
28.537914	1188.628019	16.489933
28.897983	1190.783931	16.494951
28.727998	1195.348776	16.499968
28.726709	1193.935199	16.504986
28.919094	1188.723156	16.510003
28.809245	1187.332900	16.515021
28.747588	1193.193618	16.520039
28.816632	1215.217229	16.525056
28.820451	1207.434276	16.530074
28.953304	1214.018781	16.535091
28.839319	1212.569210	16.540109
29.104103	1211.918693	16.545127
29.110873	1208.916443	16.550144
28.883427	1214.301358	16.555162
28.988022	1208.598122	16.560179
28.999385	1210.085975	16.565197
29.003342	1208.864083	16.570215
29.108360	1212.360183	16.575232
28.839629	1208.217642	16.580250
29.257335	1211.342850	16.585267
29.256861	1215.136352	16.590285
29.508201	1202.486118	16.595303
29.370045	1209.419203	16.600320
29.131153	1212.480025	16.605338
29.534734	1203.043874	16.610355
29.214029	1209.686817	16.615373
29.314196	1205.148798	16.620391
29.272189	1205.256424	16.625408
29.356523	1205.461022	16.630426
29.561642	1207.473951	16.635443
29.543015	1211.888851	16.640461
29.651331	1207.507348	16.645479
29.383806	1207.363122	16.650496
29.440596	1201.758900	16.655514
29.710988	1199.296029	16.660531
29.516578	1210.829738	16.665549
29.751306	1224.779899	16.670567
29.835016	1228.796906	16.675584
29.743684	1232.680389	16.680602
29.782147	1223.131016	16.685619
29.624854	1230.303800	16.690637
30.024559	1223.279344	16.695655
29.917320	1233.761122	16.700672
29.864899	1229.269096	16.705690
29.957629	1226.998163	16.710707
29.823179	1235.066797	16.715725
29.896751	1226.452377	16.720743
29.949518	1235.517341	16.725760
29.666022	1226.715862	16.730778
29.948586	1228.117042	16.735795
29.967208	1233.034208	16.740813
30.105294	1241.763907	16.745831
30.170969	1239.329950	16.750848
30.664204	1238.839304	16.755866
30.217703	1238.306543	16.760883
29.854216	1237.347353	16.765901
29.714340	1235.538909	16.770919
30.090254	1238.276184	16.775936
30.361444	1248.108527	16.780954
30.420942	1259.738188	16.785971
30.507991	1253.232936	16.790989
30.614313	1250.275042	16.796007
30.253919	1246.547652	16.801024
30.359228	1249.248429	16.806042
30.534303	1255.368730	16.811059
30.514202	1267.859802	16.816077
30.591853	1258.780811	16.821095
30.773096	1259.191138	16.826112
30.705927	1261.328789	16.831130
30.811390	1257.525250	16.836147
30.651247	1263.130015	16.841165
30.641115	1255.898352	16.846183
30.729801	1258.724815	16.851200
30.619476	1265.764018	16.856218
30.679660	1242.473633	16.861235
30.530879	1249.714520	16.866253
30.489156	1249.039440	16.871271
30.685499	1249.804017	16.876288
30.600640	1241.381675	16.881306
30.951681	1248.354896	16.886323
30.913109	1246.290731	16.891341
31.055759	1251.021207	16.896359
30.966337	1248.734629	16.901376
31.434258	1247.165479	16.906394
31.701898	1240.597221	16.911411
31.679843	1247.594184	16.916429
31.025005	1247.911440	16.921447
31.368405	1244.739672	16.926464
31.134380	1242.762937	16.931482
31.517331	1236.773077	16.936499
31.250675	1246.209994	16.941517
31.395545	1248.210277	16.946535
31.646200	1236.721493	16.951552
31.575643	1237.303819	16.956570
31.492294	1235.688495	16.961587
31.631343	1241.211661	16.966605
31.327310	1237.368142	16.971623
31.501768	1235.961740	16.976640
31.359713	1233.595045	16.981658
31.393096	1238.052296	16.986675
31.422951	1244.223749	16.991693
31.442328	1238.445492	16.996711
31.484788	1232.654152	17.001728
31.358940	1226.507321	17.006746
31.223836	1244.640187	17.011763
31.287376	1242.203408	17.016781
31.170397	1252.080793	17.021799
31.544603	1257.384078	17.026816
31.681541	1262.642487	17.031834
31.757036	1254.456953	17.036851
31.770854	1260.223814	17.041869
31.362640	1257.258172	17.046887
31.812150	1249.992366	17.051904
31.350714	1266.715206	17.056922
31.984101	1266.704388	17.061939
32.083962	1282.865916	17.066957
31.795295	1282.690287	17.071975
32.251485	1278.519358	17.076992
31.772440	1278.323063	17.082010
32.084212	1271.526966	17.087027
32.186858	1285.538896	17.092045
32.137564	1278.209216	17.097063
32.486474	1276.415706	17.102080
32.406803	1275.778130	17.107098
32.366009	1268.971000	17.112115
32.456965	1282.643923	17.117133
32.426523	1273.935320	17.122151
32.570205	1261.434459	17.127168
32.286232	1276.015055	17.132186
32.588348	1275.071501	17.137203
32.326964	1278.022246	17.142221
32.546126	1278.451880	17.147239
32.353697	1268.922879	17.152256
32.394352	1283.623037	17.157274
32.798680	1283.177880	17.162291
32.881531	1269.897570	17.167309
32.540068	1279.582918	17.172327
32.715285	1276.020917	17.177344
32.369574	1276.681070	17.182362
32.443467	1288.153855	17.187379
32.780602	1290.038810	17.192397
32.537367	1295.580862	17.197415
33.340839	1291.099891	17.202432
33.132081	1291.792237	17.207450
33.049714	1301.888295	17.212467
33.434894	1307.047860	17.217485
32.993562	1290.179351	17.222503
32.961275	1283.238336	17.227520
32.811219	1284.691523	17.232538
33.035108	1293.190047	17.237555
32.879073	1291.216867	17.242573
32.988003	1299.499869	17.247591
33.362966	1293.467059	17.252608
33.137917	1291.697201	17.257626
33.446991	1296.499447	17.262643
33.418391	1295.645579	17.267661
33.131114	1298.455213	17.272679
33.278793	1295.481364	17.277696
33.207159	1294.154542	17.282714
33.172405	1297.489516	17.287731
33.383768	1298.134974	17.292749
33.207774	1294.624842	17.297767
33.415045	1293.838162	17.302784
33.314587	1296.738449	17.307802
33.489905	1298.746591	17.312819
33.443999	1295.964024	17.317837
33.308107	1312.894685	17.322855
34.046425	1299.622112	17.327872
33.698781	1322.519051	17.332890
33.750303	1321.895633	17.337907
33.712651	1321.197821	17.342925
33.750379	1322.520601	17.347943
34.091058	1312.835464	17.352960
33.610599	1321.012000	17.357978
33.786686	1315.070304	17.362995
33.970122	1310.670695	17.368013
34.146329	1313.893722	17.373031
34.402691	1320.058115	17.378048
34.347458	1315.203578	17.383066
33.947771	1324.020732	17.388083
33.700999	1320.606893	17.393101
33.854544	1320.005361	17.398119
33.754485	1313.346359	17.403136
33.810928	1314.634647	17.408154
34.083992	1315.387207	17.413171
34.307713	1313.114675	17.418189
34.174987	1314.094920	17.423207
34.490330	1322.175174	17.428224
34.333593	1326.305618	17.433242
34.370039	1329.979748	17.438259
34.839146	1335.672143	17.443277
34.241489	1321.819896	17.448295
34.487898	1325.243371	17.453312
34.469190	1337.298759	17.458330
34.424113	1336.277052	17.463347
34.808902	1337.308763	17.468365
34.865345	1347.357851	17.473383
34.812650	1340.420011	17.478400
34.533359	1344.774794	17.483418
34.650405	1334.477723	17.488435
34.890218	1337.416225	17.493453
34.811193	1331.852176	17.498471
34.786716	1336.214372	17.503488
34.451592	1341.761368	17.508506
34.552758	1330.744085	17.513523
35.041093	1332.599043	17.518541
34.617872	1335.272186	17.523559
34.831116	1331.944065	17.528576
34.979521	1344.402478	17.533594
34.907778	1336.028530	17.538611
35.233862	1323.268667	17.543629
34.609929	1333.121380	17.548647
35.196442	1349.310865	17.553664
35.225381	1357.956733	17.558682
35.172286	1356.731147	17.563699
35.371948	1353.644999	17.568717
35.037366	1354.047783	17.573735
35.151819	1349.791521	17.578752
35.445425	1362.457578	17.583770
35.444444	1349.957229	17.588787
35.457826	1347.834418	17.593805
35.595675	1348.071660	17.598823
35.952825	1342.843225	17.603840
35.888782	1350.051940	17.608858
35.624191	1340.603638	17.613875
35.914077	1343.190301	17.618893
35.514062	1335.132883	17.623911
35.541266	1339.982459	17.628928
36.062376	1343.602747	17.633946
36.037445	1335.196218	17.638963
35.886872	1329.132124	17.643981
35.829363	1323.485809	17.648999
35.694892	1310.646630	17.654016
35.403072	1324.458455	17.659034
35.496423	1341.892886	17.664051
35.830073	1344.775660	17.669069
35.537267	1356.072405	17.674087
35.699036	1343.726449	17.679104
35.728527	1350.412408	17.684122
35.960869	1352.910255	17.689139
36.350007	1363.626774	17.694157
36.271863	1370.190745	17.699175
36.115757	1365.361467	17.704192
36.155782	1363.802543	17.709210
35.896285	1369.593327	17.714227
36.316043	1369.284610	17.719245
36.105882	1377.904831	17.724263
36.416302	1377.032557	17.729280
36.251489	1372.308787	17.734298
36.172988	1372.321142	17.739315
36.706552	1374.541415	17.744333
36.284425	1380.790043	17.749351
36.126987	1379.479815	17.754368
36.115700	1370.922803	17.759386
36.337874	1393.118307	17.764403
37.074748	1382.755654	17.769421
36.822053	1400.582042	17.774439
36.887744	1394.275752	17.779456
37.254752	1392.842326	17.784474
36.923984	1370.436721	17.789491
37.050795	1358.989354	17.794509
36.705956	1367.933640	17.799527
37.200405	1374.878130	17.804544
36.919744	1367.436336	17.809562
37.215393	1360.851022	17.814579
37.170904	1362.284519	17.819597
36.890126	1362.555792	17.824615
37.108756	1367.053482	17.829632
36.875253	1365.086118	17.834650
37.087837	1380.393757	17.839667
37.358162	1381.717969	17.844685
37.643022	1386.028555	17.849703
37.415526	1376.747996	17.854720
37.020466	1360.269816	17.859738
37.191502	1372.557440	17.864755
37.475814	1373.260901	17.869773
37.519031	1395.235130	17.874791
37.276931	1388.238581	17.879808
37.368997	1381.959721	17.884826
37.411498	1391.048464	17.889843
37.557261	1393.408398	17.894861
37.535261	1393.030035	17.899879
37.620059	1386.117973	17.904896
37.856569	1388.618329	17.909914
37.786194	1384.769726	17.914931
37.940375	1382.261921	17.919949
37.634109	1388.205210	17.924967
37.636884	1387.210718	17.929984
37.544241	1384.946718	17.935002
37.154402	1384.524998	17.940019
37.776739	1376.521982	17.945037
37.763527	1383.782710	17.950055
37.447867	1382.017572	17.955072
37.774165	1392.772356	17.960090
37.849847	1403.023596	17.965107
37.811063	1409.713963	17.970125
37.902559	1406.073533	17.975143
37.971172	1408.666471	17.980160
38.045741	1411.100680	17.985178
37.918849	1411.947468	17.990195
38.215595	1420.478820	17.995213
38.221298	1415.551591	18.000231
38.199281	1427.601246	18.005248
38.319781	1427.708659	18.010266
38.258073	1432.808886	18.015283
38.456798	1428.397385	18.020301
38.702567	1436.744221	18.025319
38.630546	1434.262381	18.030336
38.826084	1427.680105	18.035354
38.602311	1429.753946	18.040371
38.483229	1419.894625	18.045389
38.887877	1429.305357	18.050407
39.041987	1425.658269	18.055424
38.893392	1425.675294	18.060442
38.790459	1427.752294	18.065459
39.120387	1428.899907	18.070477
38.853031	1422.194491	18.075495
38.971574	1429.421970	18.080512
39.042549	1423.446213	18.085530
39.042802	1423.648208	18.090547
39.165069	1421.290569	18.095565
38.937217	1430.667853	18.100583
38.851027	1428.106180	18.105600
39.226114	1420.779380	18.110618
38.970975	1424.685414	18.115635
38.908382	1422.366206	18.120653
38.868947	1423.095146	18.125671
39.193507	1432.628886	18.130688
39.282592	1430.178611	18.135706
39.277514	1441.685960	18.140723
39.296123	1450.264061	18.145741
39.507348	1450.130032	18.150759
39.526175	1453.999460	18.155776
39.708393	1446.065371	18.160794
39.127594	1454.027305	18.165811
39.446892	1445.238574	18.170829
39.476482	1443.394089	18.175847
39.498007	1448.279301	18.180864
39.523515	1445.409779	18.185882
39.569639	1442.552808	18.190899
39.569311	1447.763347	18.195917
39.911798	1446.447372	18.200935
39.842707	1456.484631	18.205952
39.872657	1466.102419	18.210970
39.989329	1474.507370	18.215987
40.297439	1468.866844	18.221005
40.322490	1465.416700	18.226023
40.067337	1459.517275	18.231040
40.102998	1444.675733	18.236058
40.122093	1448.223213	18.241075
40.436098	1443.399156	18.246093
39.867077	1450.024286	18.251111
40.107847	1456.405773	18.256128
40.429007	1454.793326	18.261146
40.469183	1470.456271	18.266163
40.401264	1460.412179	18.271181
40.528219	1462.569934	18.276199
40.331084	1470.556973	18.281216
40.584086	1463.372365	18.286234
40.228673	1463.750011	18.291251
40.754787	1460.805209	18.296269
40.788231	1454.459766	18.301287
40.258511	1462.186474	18.306304
40.528257	1457.628134	18.311322
40.214596	1462.326015	18.316339
40.407457	1461.525807	18.321357
40.531422	1452.998059	18.326375
40.622304	1472.383367	18.331392
41.011489	1489.222459	18.336410
40.811997	1490.168991	18.341427
41.276058	1480.770558	18.346445
41.219053	1477.958143	18.351463
40.834027	1480.716845	18.356480
41.500239	1482.430336	18.361498
41.064069	1486.184859	18.366515
41.088423	1483.489088	18.371533
41.067891	1484.234005	18.376551
41.209752	1488.633295	18.381568
41.513643	1483.100727	18.386586
41.143630	1488.312393	18.391603
41.023977	1477.667302	18.396621
41.195857	1476.308625	18.401639
41.182596	1480.246204	18.406656
41.381790	1477.040183	18.411674
41.375630	1489.642841	18.416691
40.880993	1488.316005	18.421709
41.530697	1497.401189	18.426727
41.439354	1504.929837	18.431744
41.756132	1504.394246	18.436762
41.522577	1513.845053	18.441779
41.855234	1515.743358	18.446797
42.361213	1508.203503	18.451815
42.155615	1520.076848	18.456832
42.435736	1511.227949	18.461850
42.189816	1510.575384	18.466867
41.996712	1505.155393	18.471885
42.067535	1499.485760	18.476903
41.824432	1503.030149	18.481920
42.119103	1498.628845	18.486938
41.808748	1501.625170	18.491955
41.932730	1505.244594	18.496973
42.263591	1500.263240	18.501991
41.849564	1507.810887	18.507008
42.324323	1494.970801	18.512026
42.599657	1498.045781	18.517043
42.444591	1507.367517	18.522061
42.802141	1496.237376	18.527079
42.334550	1493.593434	18.532096
42.322394	1499.168774	18.537114
42.299422	1496.243721	18.542131
42.345872	1503.634011	18.547149
42.781259	1515.902407	18.552167
42.669272	1520.909546	18.557184
42.796534	1521.817509	18.562202
42.859473	1523.366737	18.567219
42.582129	1528.507088	18.572237
42.834983	1522.906762	18.577255
43.220888	1524.089795	18.582272
43.444239	1513.176337	18.587290
42.680192	1506.384601	18.592307
42.847836	1516.918155	18.597325
42.957792	1517.390153	18.602343
42.812646	1519.265486	18.607360
43.590354	1520.241958	18.612378
43.260463	1527.473462	18.617395
43.174417	1525.473510	18.622413
43.325508	1514.621868	18.627431
42.834761	1526.233768	18.632448
43.251229	1524.843077	18.637466
43.402152	1520.953461	18.642483
43.494809	1525.038564	18.647501
43.410796	1508.502045	18.652519
43.207031	1518.418421	18.657536
43.345749	1507.739143	18.662554
43.471552	1512.418677	18.667571
43.129067	1514.066141	18.672589
43.502605	1521.607170	18.677607
43.380567	1535.818609	18.682624
43.941993	1530.649636	18.687642
43.845753	1527.666628	18.692659
43.770767	1541.157456	18.697677
43.881499	1532.600185	18.702695
43.971309	1536.824598	18.707712
44.027480	1528.405271	18.712730
44.133072	1529.701653	18.717747
44.243598	1533.736619	18.722765
44.264394	1528.112687	18.727783
44.112521	1537.029978	18.732800
44.357999	1532.936189	18.737818
44.278881	1529.259346	18.742835
44.330457	1544.134740	18.747853
44.398265	1527.826891	18.752871
44.329928	1528.446750	18.757888
44.188651	1527.496911	18.762906
44.295059	1521.603936	18.767923
44.142720	1530.597040	18.772941
44.376440	1512.196069	18.777959
44.554445	1537.270576	18.782976
44.681317	1544.301129	18.787994
44.460092	1546.182072	18.793011
44.519161	1548.634508	18.798029
45.181866	1547.558702	18.803047
44.817398	1552.778986	18.808064
44.904359	1550.947592	18.813082
44.923354	1554.482485	18.818099
44.899152	1543.547832	18.823117
44.977340	1539.817938	18.828135
44.969219	1540.100144	18.833152
45.251703	1532.301793	18.838170
45.025631	1549.003799	18.843187
45.162807	1544.403089	18.848205
45.272986	1537.808899	18.853223
44.890274	1543.186679	18.858240
45.037921	1542.646027	18.863258
44.911470	1537.900422	18.868275
45.024674	1550.897849	18.873293
45.494534	1557.915695	18.878311
46.018719	1565.269031	18.883328
45.697483	1555.397124	18.888346
45.412407	1547.141712	18.893363
45.611275	1567.248695	18.898381
45.886412	1565.384661	18.903399
45.793927	1561.088185	18.908416
46.120458	1562.432008	18.913434
45.796033	1547.823531	18.918451
45.531893	1538.513913	18.923469
46.245515	1547.585953	18.928487
45.823825	1542.021876	18.933504
45.642631	1547.604780	18.938522
45.938316	1558.497011	18.943539
45.819721	1565.177850	18.948557
45.941760	1562.858100	18.953575
45.549746	1568.887470	18.958592
45.802618	1566.250562	18.963610
45.983849	1549.189587	18.968627
45.884342	1565.347892	18.973645
46.057511	1573.598865	18.978663
46.074365	1588.252508	18.983680
46.270226	1587.448668	18.988698
46.937166	1589.026351	18.993715
46.817781	1578.693596	18.998733
46.711316	1590.390503	19.003751
46.900156	1580.549123	19.008768
46.654340	1584.807197	19.013786
46.852089	1575.740787	19.018803
46.740026	1578.330499	19.023821
46.746827	1576.764138	19.028839
46.768342	1582.952795	19.033856
46.584452	1574.479536	19.038874
47.056608	1573.708151	19.043891
46.631019	1581.065128	19.048909
46.678045	1579.183181	19.053927
46.268335	1585.130119	19.058944
46.355787	1582.531750	19.063962
46.701377	1589.565923	19.068979
47.106179	1605.541104	19.073997
47.187100	1598.269789	19.079015
47.335479	1599.688868	19.084032
47.353159	1607.989466	19.089050
47.530509	1598.052042	19.094067
47.541527	1598.094555	19.099085
47.661511	1608.862860	19.104103
47.280984	1609.648405	19.109120
47.213294	1605.123960	19.114138
47.820903	1601.853928	19.119155
47.505563	1599.201895	19.124173
47.623111	1599.240340	19.129191
47.577997	1601.705951	19.134208
47.459240	1602.725050	19.139226
47.870150	1603.282448	19.144243
47.717173	1627.862960	19.149261
48.285900	1623.077845	19.154279
47.886805	1621.035407	19.159296
47.768316	1626.005723	19.164314
47.758070	1616.006158	19.169331
47.976658	1622.321750	19.174349
48.249428	1624.772274	19.179367
48.251040	1619.264933	19.184384
48.049941	1622.982653	19.189402
48.209519	1612.047568	19.194419
48.237465	1616.272224	19.199437
48.174675	1614.129756	19.204455
48.144093	1619.158884	19.209472
48.320071	1640.601349	19.214490
48.606598	1635.626904	19.219507
49.028751	1648.749575	19.224525
48.802662	1644.319369	19.229543
49.008785	1642.229444	19.234560
48.942285	1639.598380	19.239578
48.880036	1631.030292	19.244595
48.547025	1622.473072	19.249613
48.421430	1632.891685	19.254631
48.623602	1638.275690	19.259648
48.516616	1648.233783	19.264666
48.580732	1632.475554	19.269683
48.864734	1641.952641	19.274701
48.687944	1643.211220	19.279719
48.772206	1645.501925	19.284736
48.954509	1655.364201	19.289754
49.160763	1664.339060	19.294771
48.840508	1669.375716	19.299789
49.045706	1663.151620	19.304807
49.337574	1663.311084	19.309824
49.278166	1668.505696	19.314842
49.457576	1661.932173	19.319859
49.375657	1656.800844	19.324877
49.465467	1664.664112	19.329895
49.267667	1678.448855	19.334912
49.428715	1691.502007	19.339930
49.596623	1691.904967	19.344947
49.273374	1695.234720	19.349965
49.738162	1697.670950	19.354983
49.663518	1684.613834	19.360000
49.917498	1689.816160	19.365018
50.107510	1678.920449	19.370035
49.663184	1686.554973	19.375053
49.887089	1696.985140	19.380071
50.305527	1705.576463	19.385088
50.292365	1714.658312	19.390106
50.439834	1715.335889	19.395123
50.387179	1716.641299	19.400141
50.494030	1709.230170	19.405159
50.293251	1709.097572	19.410176
50.597679	1709.570666	19.415194
50.802785	1709.305045	19.420211
50.544950	1700.833843	19.425229
50.426390	1701.240658	19.430247
50.308475	1688.392302	19.435264
50.357832	1706.853359	19.440282
50.695719	1706.014639	19.445299
50.594118	1707.977847	19.450317
50.914932	1705.598532	19.455335
50.908865	1696.857500	19.460352
50.658915	1711.938075	19.465370
50.794754	1698.264116	19.470387
50.813394	1700.587201	19.475405
50.837210	1702.814796	19.480423
51.180079	1707.400410	19.485440
50.913600	1715.575157	19.490458
50.980059	1720.349255	19.495475
51.191655	1725.697095	19.500493
51.302787	1734.939371	19.505511
51.650295	1723.839066	19.510528
51.740520	1722.751954	19.515546
51.563443	1726.929860	19.520563
51.568414	1731.587356	19.525581
51.719976	1736.688971	19.530599
51.673305	1724.530053	19.535616
51.399053	1729.231297	19.540634
51.913881	1721.566883	19.545651
51.602310	1713.713198	19.550669
51.616161	1720.698408	19.555687
51.862334	1725.065634	19.560704
51.883925	1721.912644	19.565722
51.936304	1719.158796	19.570739
51.819748	1713.846674	19.575757
51.847423	1722.035301	19.580775
51.955728	1716.631140	19.585792
51.883724	1740.391191	19.590810
51.952183	1740.951752	19.595827
52.360894	1745.498656	19.600845
52.116410	1742.803939	19.605863
52.601844	1738.369534	19.610880
52.422969	1738.662717	19.615898
52.680201	1735.229795	19.620915
52.377764	1735.605457	19.625933
51.967612	1747.113349	19.630951
52.542579	1730.725855	19.635968
52.240646	1738.855671	19.640986
52.715179	1731.219659	19.646003
52.790149	1730.939711	19.651021
52.513776	1741.801755	19.656039
52.813239	1749.862600	19.661056
52.626742	1759.628073	19.666074
53.023500	1759.019981	19.671091
53.328812	1747.904181	19.676109
53.066739	1750.892982	19.681127
53.601264	1748.293974	19.686144
53.255370	1755.442865	19.691162
53.470482	1749.488600	19.696179
53.452074	1752.606491	19.701197
53.086472	1753.651650	19.706215
53.349048	1752.998306	19.711232
53.526954	1752.430815	19.716250
53.469432	1751.714008	19.721267
53.547860	1755.204913	19.726285
53.049690	1753.828113	19.731303
53.366558	1753.365090	19.736320
53.690332	1754.049761	19.741338
53.595265	1750.634161	19.746355
53.505818	1757.777589	19.751373
53.765987	1771.342319	19.756391
54.018671	1778.504739	19.761408
54.195912	1771.574889	19.766426
54.186955	1771.393301	19.771443
54.310248	1766.147733	19.776461
54.110526	1779.708780	19.781479
54.436814	1768.529716	19.786496
54.289296	1770.642145	19.791514
54.175114	1770.196161	19.796531
54.246368	1775.427140	19.801549
54.360755	1768.333560	19.806567
54.358335	1763.196056	19.811584
54.306035	1770.841783	19.816602
54.266358	1773.543264	19.821619
54.299980	1779.455521	19.826637
54.694363	1786.595744	19.831655
54.790451	1778.488800	19.836672
54.681790	1794.781297	19.841690
54.999522	1800.929931	19.846707
54.998005	1791.635842	19.851725
54.964467	1797.018953	19.856743
55.106807	1792.789777	19.861760
55.099546	1798.616922	19.866778
55.055291	1797.651867	19.871795
55.111778	1788.607483	19.876813
55.268472	1799.906669	19.881831
55.483157	1789.897014	19.886848
55.302734	1793.280151	19.891866
55.269224	1799.032509	19.896883
55.166585	1794.305197	19.901901
54.950233	1800.947787	19.906919
55.345105	1788.735426	19.911936
55.505700	1799.071425	19.916954
55.666990	1813.787834	19.921971
56.012012	1814.513363	19.926989
55.888510	1807.700050	19.932007
56.069180	1800.968479	19.937024
56.087399	1785.327766	19.942042
55.687314	1784.592042	19.947059
55.828656	1779.580340	19.952077
56.119307	1806.771023	19.957095
56.313642	1804.764981	19.962112
56.273563	1809.338033	19.967130
56.131624	1801.359895	19.972147
56.275962	1801.469888	19.977165
56.105777	1806.388389	19.982183
56.200416	1806.521949	19.987200
56.050011	1813.551866	19.992218
56.067227	1806.757535	19.997235
56.805299	1815.093692	20.002253
56.402615	1805.660466	20.007271
56.575031	1813.514014	20.012288
56.645639	1811.063427	20.017306
56.467316	1803.618039	20.022323
56.435018	1806.094294	20.027341
56.419426	1826.446620	20.032359
56.803122	1826.547516	20.037376
56.983785	1834.361908	20.042394
56.981611	1830.657168	20.047411
56.993039	1832.874097	20.052429
57.025332	1833.749615	20.057447
56.985968	1833.045739	20.062464
57.102490	1839.850798	20.067482
56.856434	1828.319531	20.072499
57.185445	1835.425832	20.077517
57.071761	1858.343607	20.082535
57.459535	1838.535838	20.087552
56.965561	1851.186775	20.092570
57.432000	1855.487962	20.097587
57.302477	1846.396948	20.102605
57.196218	1860.874432	20.107623
57.547022	1861.794728	20.112640
57.225990	1870.281068	20.117658
57.689326	1871.385718	20.122675
58.058026	1872.846043	20.127693
57.727607	1875.100756	20.132711
57.585742	1871.247470	20.137728
57.872194	1875.851434	20.142746
58.063822	1899.993296	20.147763
58.301631	1893.322170	20.152781
58.538963	1897.435187	20.157799
58.565649	1900.552351	20.162816
58.777009	1908.311471	20.167834
58.521749	1891.249126	20.172851
58.766087	1891.182496	20.177869
58.275679	1882.589846	20.182887
59.060694	1880.617491	20.187904
58.940160	1883.038149	20.192922
58.785108	1872.218476	20.197939
58.986087	1869.965219	20.202957
58.596548	1873.557871	20.207975
58.760236	1887.330321	20.212992
59.398710	1889.294369	20.218010
59.101534	1885.323393	20.223027
59.186974	1880.137374	20.228045
58.893776	1890.651828	20.233063
58.816662	1870.986293	20.238080
59.408035	1880.172338	20.243098
58.936220	1882.048393	20.248115
59.533188	1879.830928	20.253133
59.188236	1877.379164	20.258151
59.335716	1873.774052	20.263168
59.288337	1879.055209	20.268186
59.131409	1874.977049	20.273203
59.460694	1889.237984	20.278221
59.419410	1905.194957	20.283239
59.549269	1906.913626	20.288256
59.710352	1901.535858	20.293274
59.884286	1907.000113	20.298291
59.824178	1898.415781	20.303309
59.836864	1909.655543	20.308327
60.155295	1899.250852	20.313344
60.000620	1894.298121	20.318362
60.093604	1906.080757	20.323379
60.180865	1900.032858	20.328397
60.280138	1905.007005	20.333415
60.591434	1914.644074	20.338432
60.412027	1916.840416	20.343450
60.049615	1918.102848	20.348467
60.726561	1918.785844	20.353485
60.727879	1922.629713	20.358503
60.737357	1919.128269	20.363520
60.721263	1922.318415	20.368538
60.727755	1928.209724	20.373555
61.086531	1917.259023	20.378573
60.727984	1912.713795	20.383591
60.620975	1911.591297	20.388608
60.858553	1909.449073	20.393626
60.769280	1916.024456	20.398643
60.856906	1911.595527	20.403661
60.924286	1921.160356	20.408679
60.793199	1928.228319	20.413696
60.955715	1934.092029	20.418714
61.217276	1943.181447	20.423731
61.322710	1937.118064	20.428749
61.288282	1934.661824	20.433767
61.324595	1943.742350	20.438784
61.597144	1936.841689	20.443802
61.422654	1949.291150	20.448819
61.702673	1963.569331	20.453837
61.802958	1963.102364	20.458855
61.561898	1962.297531	20.463872
61.984013	1953.969003	20.468890
61.804341	1959.898957	20.473907
61.658383	1957.599053	20.478925
61.700191	1957.185433	20.483943
61.710939	1967.387205	20.488960
62.213676	1962.375640	20.493978
62.491114	1983.313437	20.498995
62.629547	1983.061414	20.504013
62.539273	1978.385768	20.509031
62.430312	1978.601724	20.514048
62.617356	1967.895665	20.519066
62.782868	1967.983405	20.524083
63.047331	1964.009628	20.529101
63.021956	1966.099787	20.534119
63.258192	1958.526263	20.539136
63.264858	1949.963005	20.544154
63.092556	1947.989143	20.549171
62.866906	1934.955503	20.554189
63.209254	1938.061089	20.559207
63.248546	1943.963044	20.564224
63.054017	1927.030015	20.569242
63.458507	1932.158334	20.574259
63.345909	1934.943853	20.579277
63.350809	1938.462094	20.584295
63.422861	1947.019436	20.589312
63.689214	1947.173434	20.594330
63.743862	1962.114971	20.599347
63.523261	1950.093611	20.604365
63.497425	1947.336202	20.609383
63.399927	1963.734408	20.614400
63.636569	1959.622971	20.619418
63.511124	1967.371765	20.624435
63.312472	1967.447129	20.629453
63.684495	1968.480879	20.634471
63.826228	1971.248649	20.639488
63.701681	1972.499065	20.644506
64.079499	1987.377366	20.649523
63.948361	1982.790178	20.654541
64.010225	1988.641271	20.659559
64.056601	1988.069133	20.664576
64.252642	1991.216587	20.669594
63.880980	1992.584622	20.674611
64.068478	1994.010227	20.679629
64.691889	2004.977626	20.684647
64.344264	2013.837455	20.689664
64.647774	2010.422479	20.694682
64.485143	2007.910571	20.699699
64.621013	2006.803667	20.704717
64.647793	1999.259786	20.709735
64.547589	2011.666091	20.714752
64.975340	2012.167213	20.719770
65.167916	2025.452372	20.724787
65.362085	2029.995091	20.729805
65.520905	2027.868349	20.734823
65.306535	2030.310040	20.739840
65.327386	2034.838886	20.744858
65.376315	2034.932269	20.749875
65.532543	2036.921394	20.754893
65.624505	2041.565342	20.759911
65.532632	2038.376421	20.764928
66.165140	2030.090638	20.769946
66.259961	2043.548928	20.774963
65.663312	2040.947214	20.779981
65.790762	2037.020136	20.784999
65.726227	2040.063247	20.790016
65.749513	2034.378801	20.795034
66.009817	2038.516656	20.800051
65.949803	2030.168950	20.805069
66.066976	2033.117314	20.810087
65.993574	2038.721354	20.815104
66.013560	2039.210619	20.820122
66.235939	2055.082231	20.825139
66.253585	2055.549771	20.830157
66.442635	2054.090524	20.835175
66.629830	2050.141459	20.840192
66.236584	2044.020461	20.845210
66.200356	2053.068223	20.850227
66.622399	2073.970847	20.855245
67.438989	2072.391186	20.860263
67.321206	2079.772728	20.865280
66.938932	2061.748593	20.870298
66.990465	2066.891223	20.875315
67.086183	2072.572926	20.880333
67.176695	2074.559727	20.885351
67.070903	2074.415400	20.890368
67.468947	2063.174415	20.895386
67.265609	2065.560730	20.900403
67.156469	2062.068375	20.905421
67.548246	2072.122141	20.910439
67.293621	2062.955936	20.915456
67.712894	2065.039561	20.920474
67.512930	2061.959096	20.925491
67.754129	2056.224721	20.930509
68.119334	2068.346694	20.935527
67.976778	2078.253789	20.940544
67.727950	2072.239552	20.945562
67.892943	2080.640375	20.950579
67.663134	2082.964563	20.955597
68.012000	2086.302701	20.960615
67.875868	2089.347570	20.965632
68.162258	2081.712483	20.970650
67.805300	2091.915129	20.975667
68.208181	2108.402340	20.980685
68.907311	2106.449731	20.985703
68.603787	2118.780660	20.990720
69.087040	2114.302321	20.995738
68.918320	2105.154196	21.000755
68.564259	2096.735754	21.005773
68.897185	2093.486580	21.010791
69.112217	2108.459920	21.015808
69.321937	2111.829331	21.020826
69.083706	2099.362474	21.025843
68.705519	2096.666559	21.030861
69.380538	2109.813074	21.035879
68.904798	2107.520634	21.040896
69.223560	2102.253811	21.045914
69.195845	2096.839287	21.050931
69.454295	2099.566697	21.055949
69.517833	2099.294847	21.060967
69.211780	2109.628392	21.065984
69.554834	2102.154846	21.071002
69.506761	2106.467273	21.076019
69.451805	2122.196191	21.081037
69.946488	2135.898038	21.086055
69.758976	2138.897312	21.091072
69.978073	2132.490982	21.096090
69.820344	2133.844445	21.101107
69.812143	2130.011189	21.106125
69.985141	2132.663624	21.111143
69.990473	2134.891013	21.116160
70.140048	2138.014213	21.121178
70.753645	2148.131105	21.126195
70.486256	2146.102686	21.131213
70.887246	2141.166978	21.136231
70.689778	2142.918018	21.141248
70.538122	2146.445048	21.146266
70.799051	2147.849693	21.151283
70.740764	2140.959758	21.156301
71.088508	2136.935023	21.161319
70.900884	2141.439750	21.166336
70.983797	2140.034998	21.171354
71.080795	2139.312902	21.176371
70.908580	2145.058699	21.181389
70.820300	2145.577553	21.186407
70.994756	2160.705628	21.191424
71.100228	2165.691501	21.196442
71.064221	2171.090892	21.201459
71.288463	2167.861889	21.206477
71.639121	2168.697012	21.211495
71.510696	2173.419708	21.216512
71.616521	2191.591530	21.221530
71.917874	2193.794639	21.226547
71.789293	2193.486610	21.231565
72.303149	2191.935435	21.236583
72.265576	2191.063994	21.241600
72.208677	2189.731640	21.246618
72.181106	2187.877098	21.251635
71.841798	2196.319114	21.256653
72.343881	2188.820615	21.261671
72.135122	2186.009772	21.266688
72.260659	2189.550190	21.271706
71.832845	2199.322150	21.276723
72.041465	2207.889780	21.281741
72.916994	2211.372663	21.286759
72.791365	2216.057059	21.291776
73.091325	2216.347817	21.296794
73.017127	2207.295292	21.301811
72.941201	2217.087875	21.306829
72.985954	2200.315929	21.311847
73.164657	2212.296792	21.316864
73.353758	2202.199391	21.321882
73.250595	2198.286317	21.326899
73.099083	2209.854974	21.331917
73.600248	2197.575186	21.336935
73.471298	2204.841755	21.341952
73.321682	2197.016134	21.346970
73.537522	2200.122651	21.351987
73.507356	2203.457074	21.357005
73.711553	2200.998128	21.362023
73.628717	2208.153324	21.367040
73.753976	2216.740332	21.372058
73.954160	2223.589238	21.377075
73.897026	2227.215093	21.382093
74.332841	2221.462799	21.387111
74.120567	2226.530032	21.392128
73.757029	2219.309165	21.397146
74.213580	2225.300486	21.402163
73.709661	2222.277084	21.407181
73.857849	2231.599025	21.412199
74.025502	2249.224687	21.417216
74.328819	2245.582461	21.422234
74.498493	2235.869968	21.427251
74.432696	2261.523375	21.432269
75.037329	2261.599128	21.437287
74.710973	2266.141402	21.442304
75.017804	2272.998867	21.447322
75.351308	2271.823110	21.452339
75.043654	2267.171978	21.457357
75.103801	2264.710344	21.462375
75.312266	2270.390225	21.467392
75.359988	2257.086283	21.472410
75.624998	2268.722275	21.477427
75.388572	2262.033788	21.482445
75.435824	2268.692060	21.487463
75.328348	2264.211554	21.492480
75.619142	2282.629066	21.497498
75.566274	2287.125341	21.502515
75.711532	2287.774882	21.507533
75.746936	2283.505536	21.512551
76.242135	2287.871757	21.517568
76.065671	2293.129075	21.522586
76.172367	2281.778954	21.527603
75.970315	2278.155934	21.532621
76.277863	2289.356049	21.537639
76.203335	2308.531473	21.542656
76.283077	2316.466039	21.547674
76.614386	2302.158185	21.552691
76.190280	2309.196461	21.557709
76.511601	2304.178508	21.562727
76.544274	2306.439508	21.567744
76.899036	2316.612830	21.572762
77.162356	2323.511849	21.577779
77.307756	2333.285599	21.582797
77.314969	2325.766739	21.587815
77.354087	2326.679086	21.592832
77.466942	2334.002504	21.597850
77.569102	2319.544329	21.602867
77.563883	2312.737541	21.607885
77.411764	2300.294925	21.612903
77.554683	2314.389722	21.617920
77.418684	2315.443123	21.622938
77.546536	2311.796814	21.627955
77.615056	2317.381861	21.632973
77.744609	2314.180291	21.637991
77.767720	2312.696525	21.643008
77.763611	2311.791430	21.648026
78.261248	2313.430426	21.653043
77.864243	2321.401815	21.658061
77.586944	2327.419776	21.663079
77.847249	2335.007297	21.668096
77.766238	2338.081445	21.673114
78.417852	2332.487827	21.678131
78.276824	2334.836010	21.683149
78.349053	2348.392751	21.688167
78.430950	2359.928092	21.693184
78.512419	2358.851782	21.698202
78.686790	2362.195219	21.703219
78.730754	2360.468319	21.708237
78.649502	2368.084119	21.713255
78.696599	2370.352335	21.718272
78.640883	2380.328049	21.723290
79.179569	2378.100722	21.728307
78.880956	2386.347085	21.733325
79.166192	2386.608592	21.738343
79.327484	2379.135004	21.743360
79.421978	2391.978169	21.748378
79.824081	2402.166216	21.753395
79.885655	2407.966994	21.758413
80.110265	2407.013435	21.763431
80.153396	2405.886320	21.768448
80.346321	2402.687430	21.773466
80.409477	2388.655071	21.778483
80.195648	2379.292946	21.783501
79.935942	2372.346109	21.788519
80.066402	2379.729910	21.793536
80.545136	2389.050643	21.798554
80.623082	2391.389775	21.803571
80.697379	2397.179088	21.808589
80.381788	2398.339533	21.813607
80.432339	2398.615717	21.818624
80.474315	2397.447754	21.823642
80.807467	2395.924874	21.828659
80.393560	2400.288377	21.833677
80.890438	2410.297462	21.838695
80.833288	2420.361794	21.843712
80.774669	2423.748058	21.848730
81.023347	2423.393542	21.853747
80.664254	2422.641897	21.858765
80.572159	2430.783334	21.863783
81.089357	2444.396676	21.868800
81.119692	2458.174679	21.873818
81.628824	2449.024327	21.878835
81.413806	2458.068744	21.883853
81.605855	2460.257451	21.888871
81.966350	2470.953876	21.893888
81.665092	2473.153596	21.898906
82.110685	2465.834264	21.903923
82.061647	2464.162955	21.908941
81.784599	2472.017777	21.913959
82.407822	2470.439976	21.918976
81.924772	2479.494836	21.923994
82.679480	2486.607292	21.929011
82.647763	2503.301828	21.934029
82.547556	2495.389432	21.939047
83.090544	2495.266543	21.944064
82.617242	2487.387356	21.949082
82.990572	2480.110902	21.954099
83.188008	2479.224719	21.959117
82.826366	2484.634193	21.964135
83.001818	2482.829871	21.969152
82.903249	2491.306897	21.974170
83.229462	2485.076183	21.979187
83.074950	2488.736283	21.984205
83.166068	2487.604801	21.989223
83.485192	2497.048436	21.994240
83.391112	2507.446838	21.999258
83.737686	2500.038854	22.004275
83.413168	2505.789690	22.009293
83.651140	2514.030946	22.014311
83.815754	2499.278791	22.019328
83.675173	2509.703417	22.024346
83.981397	2507.544056	22.029363
83.685380	2521.912933	22.034381
84.011662	2531.576393	22.039399
84.066805	2532.502019	22.044416
83.987157	2531.776022	22.049434
84.435879	2530.178215	22.054451
84.496695	2530.446480	22.059469
84.506292	2529.274113	22.064487
84.573503	2538.552091	22.069504
84.775037	2549.778447	22.074522
84.882571	2551.295529	22.079539
85.134168	2544.473665	22.084557
85.381826	2548.522094	22.089575
85.501548	2549.601722	22.094592
84.945808	2553.978014	22.099610
85.349416	2551.345753	22.104627
85.471865	2555.095032	22.109645
85.321307	2560.676605	22.114663
85.561300	2547.781025	22.119680
85.493455	2546.103186	22.124698
85.631258	2542.228031	22.129715
85.504700	2551.962450	22.134733
85.590049	2567.073268	22.139751
86.069983	2562.263947	22.144768
86.144269	2568.507798	22.149786
86.411327	2570.949882	22.154803
86.213157	2569.371363	22.159821
86.076778	2575.449387	22.164839
86.311301	2567.509765	22.169856
86.297523	2566.492552	22.174874
86.848283	2595.518417	22.179891
86.229010	2598.493885	22.184909
86.462539	2598.741404	22.189927
86.709728	2591.547791	22.194944
86.800537	2600.014134	22.199962
87.306378	2592.559067	22.204979
87.341031	2593.427941	22.209997
86.766804	2598.858131	22.215015
86.931177	2604.898513	22.220032
87.477466	2605.892376	22.225050
87.397225	2616.395981	22.230067
87.364443	2616.836719	22.235085
87.473288	2618.940642	22.240103
87.744621	2615.401193	22.245120
87.754978	2616.984004	22.250138
88.044953	2613.779341	22.255155
87.853594	2623.798535	22.260173
88.191921	2628.624965	22.265191
88.139047	2633.339100	22.270208
88.086669	2639.413454	22.275226
88.220494	2641.147354	22.280243
88.538428	2632.897959	22.285261
88.393340	2628.603154	22.290279
88.819023	2625.225733	22.295296
88.332758	2638.115878	22.300314
88.172417	2634.830269	22.305331
88.470927	2648.115074	22.310349
88.442473	2655.716411	22.315367
88.728518	2644.129657	22.320384
88.727140	2656.786039	22.325402
88.800907	2665.779003	22.330419
88.965063	2675.250167	22.335437
89.243788	2680.657212	22.340455
89.694269	2679.412604	22.345472
89.185716	2677.879547	22.350490
89.531273	2680.220976	22.355507
89.332823	2674.280702	22.360525
89.822418	2693.560678	22.365543
89.879979	2698.629954	22.370560
90.055851	2703.267239	22.375578
90.046552	2707.826228	22.380595
90.008150	2698.985621	22.385613
89.703400	2717.762002	22.390631
90.574900	2698.900094	22.395648
90.462089	2698.873638	22.400666
90.474868	2695.399931	22.405683
90.545989	2700.710105	22.410701
90.657331	2699.960491	22.415719
90.518873	2708.693204	22.420736
90.849757	2715.376640	22.425754
90.664179	2705.492310	22.430771
90.886936	2703.996169	22.435789
91.261251	2708.889575	22.440807
91.412748	2706.063236	22.445824
91.709494	2709.848363	22.450842
91.574025	2712.173631	22.455859
91.691259	2704.987708	22.460877
91.479236	2704.171978	22.465895
91.819234	2701.395011	22.470912
91.783599	2707.324737	22.475930
91.596016	2721.967150	22.480947
91.942871	2717.232293	22.485965
91.822385	2729.563367	22.490983
92.412209	2731.364705	22.496000
92.123688	2731.141690	22.501018
92.147306	2727.577907	22.506035
92.259628	2730.214688	22.511053
92.401290	2734.235579	22.516071
92.587573	2741.995835	22.521088
92.410432	2756.059063	22.526106
92.470245	2748.717999	22.531123
92.807295	2758.465111	22.536141
92.568672	2759.761859	22.541159
92.917010	2764.675130	22.546176
92.980476	2775.465617	22.551194
93.085500	2782.440112	22.556211
93.488748	2782.058218	22.561229
93.632984	2783.285515	22.566247
93.851055	2790.740976	22.571264
93.706614	2778.303138	22.576282
93.231368	2781.312880	22.581299
93.578178	2776.246618	22.586317
93.789937	2784.997091	22.591335
93.941223	2789.865494	22.596352
93.855247	2793.237177	22.601370
93.657220	2793.706964	22.606387
94.150385	2790.479904	22.611405
93.900727	2798.879749	22.616423
94.074818	2804.094918	22.621440
94.338850	2809.403306	22.626458
94.185033	2816.573020	22.631475
94.618108	2814.895580	22.636493
94.704155	2828.832415	22.641511
95.109941	2835.567284	22.646528
95.125018	2838.184598	22.651546
95.409710	2851.339159	22.656563
95.383022	2835.527822	22.661581
95.147241	2836.476951	22.666599
95.385944	2833.879955	22.671616
95.402094	2837.772194	22.676634
95.504015	2839.198651	22.681651
95.598330	2835.317622	22.686669
95.728018	2835.076427	22.691687
95.755103	2833.557278	22.696704
95.656021	2836.419722	22.701722
95.570503	2851.270337	22.706739
95.964807	2860.238428	22.711757
96.079482	2857.746077	22.716775
96.011710	2853.991435	22.721792
95.941844	2860.838709	22.726810
96.087753	2875.394280	22.731827
96.654612	2868.645993	22.736845
97.147395	2878.596016	22.741863
97.219847	2875.905126	22.746880
97.184581	2875.538278	22.751898
97.164293	2879.202677	22.756915
97.363280	2870.968654	22.761933
97.307556	2883.302311	22.766951
97.296093	2872.737281	22.771968
97.431392	2877.734460	22.776986
97.543055	2875.712849	22.782003
97.780494	2868.381781	22.787021
97.476867	2870.351517	22.792039
97.354327	2866.690671	22.797056
97.890324	2871.227392	22.802074
97.545974	2897.786984	22.807091
97.660428	2890.822355	22.812109
98.106536	2894.517841	22.817127
97.990818	2895.167263	22.822144
98.140845	2893.581504	22.827162
98.333965	2917.175326	22.832179
98.769865	2919.272231	22.837197
98.737553	2916.632466	22.842215
98.758205	2923.276211	22.847232
98.887088	2917.382415	22.852250
98.820708	2919.819976	22.857267
98.875649	2908.973089	22.862285
99.181823	2911.238658	22.867303
99.339361	2914.941484	22.872320
99.423321	2922.582133	22.877338
99.558365	2938.139968	22.882355
99.725814	2935.913926	22.887373
99.662880	2947.702737	22.892391
100.038214	2943.111701	22.897408
99.815000	2942.215652	22.902426
99.171878	2947.274839	22.907443
99.619145	2936.047695	22.912461
99.742310	2947.788412	22.917479
99.957210	2958.179696	22.922496
100.090161	2966.595423	22.927514
99.714487	2968.153528	22.932531
100.293382	2973.693536	22.937549
100.281260	2982.614898	22.942567
100.301940	2979.158836	22.947584
100.541610	2986.181751	22.952602
100.608487	2991.224400	22.957619
100.980410	3001.581639	22.962637
101.184120	3001.010069	22.967655
101.335708	3009.987857	22.972672
101.487013	3003.929553	22.977690
101.563235	3016.574031	22.982707
101.837824	2995.233030	22.987725
101.468593	3003.777952	22.992743
101.732559	3003.468375	22.997760
101.675096	3003.032409	23.002778
101.353900	3004.859727	23.007795
101.639935	3019.409241	23.012813
102.178300	3026.716777	23.017831
101.736616	3033.101596	23.022848
102.145325	3035.515239	23.027866
102.117145	3029.096834	23.032883
102.187031	3035.818124	23.037901
102.437388	3048.192314	23.042919
102.326412	3054.743107	23.047936
102.863369	3052.045696	23.052954
102.476024	3054.489375	23.057971
103.138259	3044.068035	23.062989
103.480936	3056.494048	23.068007
103.505842	3067.672652	23.073024
104.124750	3052.848870	23.078042
103.621242	3048.202968	23.083059
103.498368	3032.589587	23.088077
103.682113	3037.964278	23.093095
103.717050	3040.837319	23.098112
104.145157	3050.636605	23.103130
104.007723	3055.805968	23.108147
104.153813	3054.621651	23.113165
104.246511	3053.126921	23.118183
104.003656	3049.393357	23.123200
104.487892	3046.975641	23.128218
104.550741	3050.241993	23.133235
104.558334	3050.515449	23.138253
104.442663	3047.427919	23.143271
104.397668	3063.525375	23.148288
104.705374	3060.393605	23.153306
105.045077	3074.499199	23.158323
104.996410	3073.784107	23.163341
105.211153	3071.888354	23.168359
105.072071	3075.864933	23.173376
105.313959	3067.134886	23.178394
105.387090	3091.524163	23.183411
105.570488	3084.558127	23.188429
105.862071	3095.505595	23.193447
105.713864	3097.422600	23.198464
106.028843	3093.857283	23.203482
105.450873	3097.470226	23.208499
106.003255	3101.133324	23.213517
106.123887	3102.345405	23.218535
105.749242	3111.440407	23.223552
105.934045	3108.078543	23.228570
105.807343	3117.860633	23.233587
105.817591	3128.214641	23.238605
105.984064	3140.349539	23.243623
106.468035	3157.497289	23.248640
106.639835	3157.268430	23.253658
106.793191	3160.154500	23.258675
106.987369	3180.797431	23.263693
107.377091	3194.058881	23.268711
107.278022	3191.754627	23.273728
107.907995	3187.745413	23.278746
107.718023	3188.109792	23.283763
107.677926	3182.008822	23.288781
108.269422	3176.291806	23.293799
107.877420	3180.759374	23.298816
107.926141	3171.456700	23.303834
108.255498	3175.912251	23.308851
108.256855	3186.305560	23.313869
108.594191	3192.757759	23.318887
108.143683	3203.935181	23.323904
108.263883	3191.263066	23.328922
108.433138	3196.769480	23.333939
108.298701	3197.649093	23.338957
108.878441	3209.460480	23.343975
108.977436	3214.829564	23.348992
109.244326	3219.168663	23.354010
109.136707	3214.722660	23.359027
109.491691	3210.466150	23.364045
109.562194	3219.592464	23.369063
109.560403	3221.959979	23.374080
109.759289	3203.477519	23.379098
109.863266	3217.695907	23.384115
110.015818	3212.789365	23.389133
109.672244	3211.031569	23.394151
109.712353	3234.132156	23.399168
110.231393	3244.008832	23.404186
110.584159	3244.834211	23.409203
110.653520	3241.493565	23.414221
110.590063	3244.918616	23.419239
110.633268	3245.151777	23.424256
110.553270	3234.628834	23.429274
110.464001	3239.654985	23.434291
110.547943	3252.472012	23.439309
110.698977	3252.953404	23.444327
110.688418	3266.230277	23.449344
110.867429	3269.330126	23.454362
110.906210	3280.336251	23.459379
111.097240	3289.967654	23.464397
111.377077	3285.520900	23.469415
111.262738	3287.457869	23.474432
111.407746	3304.482115	23.479450
111.786011	3307.541284	23.484467
111.940751	3315.578168	23.489485
111.923788	3310.237344	23.494503
111.945386	3330.598171	23.499520
112.411115	3334.451644	23.504538
112.661798	3330.170416	23.509555
112.575304	3337.339257	23.514573
112.974993	3328.767425	23.519591
112.736262	3339.422531	23.524608
112.996983	3333.662601	23.529626
113.187071	3343.044837	23.534643
113.386785	3349.850061	23.539661
113.614841	3345.291467	23.544679
113.850917	3356.973730	23.549696
113.814251	3345.077273	23.554714
113.999965	3342.901977	23.559731
113.894443	3351.999123	23.564749
114.240207	3346.746648	23.569767
114.130365	3342.679713	23.574784
113.999788	3340.961128	23.579802
114.201718	3347.611347	23.584819
114.025387	3342.484857	23.589837
114.010052	3335.600361	23.594855
114.335218	3357.649600	23.599872
114.546726	3361.391408	23.604890
114.554474	3364.347667	23.609907
114.896553	3373.949139	23.614925
115.376789	3363.126880	23.619943
115.126427	3367.749053	23.624960
115.324569	3367.228845	23.629978
115.432056	3382.343191	23.634995
115.101740	3391.459794	23.640013
115.020382	3391.990224	23.645031
115.320749	3390.743840	23.650048
115.307772	3401.802335	23.655066
115.402455	3408.747131	23.660083
115.543117	3416.726296	23.665101
115.746723	3418.746029	23.670119
115.853564	3441.138891	23.675136
116.295317	3438.879282	23.680154
116.345180	3444.824261	23.685171
116.207301	3444.239913	23.690189
116.981022	3440.962474	23.695207
116.642963	3457.437604	23.700224
116.985310	3452.403417	23.705242
117.352066	3456.057796	23.710259
117.112085	3463.856740	23.715277
117.353071	3450.976142	23.720295
116.905813	3457.320950	23.725312
117.371173	3450.392662	23.730330
117.798373	3459.074992	23.735347
117.593970	3473.105174	23.740365
118.144489	3474.578183	23.745383
117.954383	3480.750148	23.750400
117.814973	3476.170185	23.755418
118.180663	3469.560508	23.760435
118.124755	3484.817321	23.765453
118.517116	3473.178662	23.770471
118.452193	3493.853075	23.775488
118.752346	3486.205773	23.780506
118.588189	3491.568824	23.785523
118.627040	3494.315073	23.790541
118.819458	3490.071342	23.795559
118.922654	3503.295848	23.800576
119.308377	3516.482413	23.805594
119.470540	3514.815792	23.810611
119.247316	3525.437016	23.815629
119.703414	3521.224562	23.820647
119.724562	3527.524416	23.825664
119.954487	3515.608174	23.830682
120.029135	3518.377226	23.835699
120.171991	3541.215918	23.840717
120.454640	3543.996574	23.845735
120.248779	3533.572083	23.850752
120.070021	3540.985870	23.855770
120.123632	3537.300445	23.860787
120.502884	3551.674815	23.865805
120.540457	3553.130349	23.870823
121.080760	3556.454555	23.875840
120.988424	3559.054083	23.880858
121.358350	3553.605230	23.885875
121.289291	3557.321596	23.890893
121.554847	3567.143475	23.895911
121.901194	3578.496133	23.900928
121.458704	3580.415105	23.905946
122.045879	3575.942224	23.910963
122.187323	3580.657726	23.915981
121.843321	3576.933585	23.920999
121.998477	3577.098710	23.926016
122.317013	3570.108159	23.931034
122.333920	3585.959660	23.936051
122.458620	3602.356109	23.941069
122.667765	3596.733584	23.946087
122.341481	3595.837867	23.951104
122.371645	3599.926923	23.956122
122.772457	3610.526180	23.961139
122.669298	3617.240079	23.966157
122.436037	3626.764539	23.971175
122.985814	3639.584611	23.976192
122.518673	3645.266617	23.981210
123.119661	3648.019510	23.986227
123.137406	3683.572674	23.991245
123.699878	3675.710598	23.996263
124.413209	3675.693587	24.001280
124.472153	3670.751085	24.006298
124.686180	3662.422813	24.011315
124.633308	3662.838317	24.016333
124.940898	3659.577054	24.021351
124.777917	3654.240067	24.026368
125.069805	3658.865737	24.031386
125.220529	3650.585264	24.036403
125.024391	3658.115448	24.041421
125.343059	3659.208164	24.046439
125.639797	3659.480517	24.051456
125.233568	3664.755291	24.056474
125.670423	3675.326846	24.061491
125.483536	3676.969059	24.066509
125.449403	3674.752415	24.071527
125.810781	3677.438694	24.076544
125.940905	3672.945862	24.081562
126.054719	3664.301876	24.086579
125.997214	3671.845066	24.091597
126.333187	3685.150020	24.096615
126.102354	3694.298533	24.101632
125.997643	3695.132481	24.106650
126.546358	3702.615427	24.111667
126.622060	3714.398800	24.116685
126.599096	3724.051337	24.121703
126.671786	3710.003832	24.126720
126.930860	3713.561507	24.131738
127.334793	3730.981163	24.136755
127.284373	3746.587690	24.141773
127.705674	3739.318999	24.146791
127.574821	3742.410663	24.151808
127.472345	3752.242957	24.156826
127.817404	3763.842128	24.161843
128.093942	3771.812788	24.166861
128.057117	3769.849060	24.171879
128.899698	3768.337793	24.176896
128.200641	3772.190780	24.181914
128.545386	3764.539531	24.186931
128.520327	3773.892571	24.191949
128.481291	3783.190992	24.196967
128.860036	3786.856187	24.201984
128.642357	3789.147126	24.207002
129.275814	3798.406480	24.212019
129.478807	3813.225310	24.217037
129.479710	3816.618291	24.222055
129.432216	3813.115936	24.227072
129.435377	3814.557944	24.232090
129.672223	3823.030391	24.237107
129.774316	3835.052746	24.242125
130.225207	3834.890628	24.247143
130.325098	3831.863881	24.252160
130.165407	3836.399371	24.257178
130.159911	3844.679382	24.262195
130.233594	3854.089590	24.267213
130.528122	3856.874747	24.272231
130.874192	3865.393229	24.277248
130.617538	3881.919117	24.282266
131.077385	3875.180913	24.287283
131.251638	3882.277556	24.292301
131.327539	3893.666470	24.297319
131.795854	3903.987035	24.302336
131.393604	3905.767168	24.307354
132.036015	3901.626442	24.312371
131.853580	3905.682591	24.317389
132.154529	3901.828931	24.322407
131.896495	3911.063880	24.327424
132.183605	3919.708410	24.332442
132.314159	3926.123830	24.337459
132.423676	3925.011471	24.342477
132.734613	3936.887546	24.347495
132.912782	3936.796561	24.352512
132.762163	3951.405770	24.357530
132.904382	3945.822030	24.362547
132.911515	3958.133948	24.367565
133.203337	3975.530371	24.372583
133.564888	3973.194885	24.377600
133.496700	3991.196934	24.382618
133.546148	3980.880535	24.387635
133.777811	3979.202984	24.392653
133.630007	3988.180819	24.397671
133.871960	3992.861744	24.402688
133.900402	3999.542541	24.407706
134.076202	4002.267412	24.412723
134.196455	4023.087019	24.417741
134.605709	4028.398269	24.422759
135.076028	4028.100538	24.427776
134.674525	4033.289455	24.432794
134.654371	4032.402569	24.437811
134.914549	4039.334306	24.442829
135.011328	4049.804697	24.447847
135.378201	4052.439670	24.452864
135.255337	4073.108040	24.457882
136.025826	4072.813784	24.462899
135.788239	4081.764698	24.467917
135.971279	4075.786287	24.472935
136.178173	4074.052637	24.477952
136.297073	4094.159195	24.482970
136.771579	4091.695524	24.487987
136.559748	4097.451301	24.493005
136.671098	4102.727179	24.498023
136.797467	4100.842010	24.503040
137.000294	4097.836969	24.508058
137.122274	4106.867288	24.513075
137.352680	4118.402583	24.518093
137.442496	4117.788852	24.523111
137.480439	4114.020542	24.528128
137.525724	4119.941210	24.533146
138.032346	4127.866512	24.538163
138.049232	4140.770429	24.543181
137.850957	4150.198146	24.548199
138.046473	4143.857929	24.553216
138.282856	4149.000602	24.558234
138.782862	4161.825688	24.563251
138.869894	4164.428765	24.568269
138.669943	4161.385812	24.573287
139.181450	4159.976886	24.578304
138.915535	4168.705020	24.583322
138.920706	4162.277830	24.588339
139.280253	4171.027919	24.593357
139.401137	4180.115262	24.598375
139.696076	4184.030398	24.603392
139.880612	4179.557325	24.608410
139.885838	4190.979594	24.613427
140.168036	4198.356151	24.618445
140.243358	4201.074699	24.623463
140.501928	4203.755070	24.628480
140.391647	4211.010050	24.633498
140.346037	4203.520778	24.638515
140.265474	4206.715116	24.643533
140.521704	4222.412892	24.648551
140.856033	4233.499551	24.653568
140.985836	4236.938701	24.658586
140.805481	4242.162471	24.663603
141.162621	4258.513630	24.668621
141.284487	4264.356063	24.673639
141.666179	4276.076081	24.678656
141.588389	4288.262645	24.683674
141.684589	4274.668700	24.688691
142.120888	4291.774498	24.693709
142.074504	4295.026624	24.698727
142.285761	4308.099063	24.703744
142.273658	4306.715343	24.708762
142.543510	4313.348966	24.713779
143.225208	4324.356008	24.718797
142.819733	4328.046326	24.723815
143.116407	4327.220264	24.728832
142.813563	4326.197735	24.733850
143.331847	4333.919290	24.738867
143.207847	4349.367416	24.743885
143.546915	4349.917230	24.748903
143.632421	4352.369065	24.753920
143.742431	4356.483659	24.758938
143.877778	4372.143687	24.763955
144.057460	4373.965266	24.768973
144.188519	4378.101818	24.773991
144.251565	4376.299139	24.779008
144.433294	4397.333652	24.784026
144.468110	4404.524944	24.789043
145.049180	4393.373790	24.794061
144.817741	4406.682946	24.799079
145.158068	4411.563207	24.804096
145.410302	4420.298665	24.809114
145.602926	4424.463461	24.814131
146.234326	4414.645899	24.819149
145.763505	4416.881882	24.824167
146.324782	4416.033301	24.829184
146.330559	4439.825755	24.834202
146.603383	4443.731787	24.839219
146.878263	4440.535484	24.844237
146.988074	4443.128720	24.849255
146.896935	4433.260211	24.854272
146.867433	4434.603223	24.859290
146.954066	4433.948947	24.864307
147.084339	4435.386872	24.869325
147.323046	4446.381323	24.874343
147.502317	4455.658513	24.879360
147.798335	4462.786811	24.884378
147.924720	4458.316467	24.889395
147.882972	4465.336703	24.894413
147.629374	4472.497451	24.899431
148.191671	4485.657063	24.904448
148.324715	4480.270297	24.909466
148.449587	4485.029666	24.914483
148.111465	4490.830604	24.919501
148.443863	4505.165729	24.924519
148.589823	4497.681044	24.929536
148.733509	4516.767808	24.934554
148.931907	4521.790279	24.939571
149.219024	4520.211312	24.944589
149.104428	4522.189485	24.949607
149.697219	4529.744785	24.954624
150.091355	4537.564789	24.959642
149.891724	4543.265135	24.964659
150.121057	4533.459996	24.969677
150.157858	4563.838455	24.974695
150.490325	4560.936131	24.979712
150.749636	4569.859941	24.984730
150.344200	4572.799061	24.989747
150.767051	4575.362212	24.994765
150.665789	4582.742186	24.999783
150.993146	4585.998942	25.004800
151.178581	4593.646496	25.009818
151.076557	4612.172123	25.014835
151.314576	4611.509906	25.019853
151.367299	4616.886657	25.024871
151.538304	4631.588066	25.029888
151.773295	4644.893766	25.034906
152.175618	4643.404060	25.039923
152.225075	4658.948377	25.044941
152.577205	4663.981525	25.049959
152.593671	4666.182230	25.054976
152.713738	4672.002981	25.059994
152.873296	4661.918308	25.065011
153.244184	4674.981785	25.070029
153.377607	4686.163327	25.075047
153.804518	4690.240976	25.080064
153.931153	4694.902272	25.085082
153.735980	4694.244789	25.090099
154.020241	4692.618907	25.095117
153.483278	4693.893084	25.100135
154.043259	4703.593701	25.105152
154.064565	4713.006247	25.110170
154.304036	4725.698944	25.115187
153.993080	4713.282703	25.120205
154.280977	4736.671507	25.125223
154.839003	4733.607558	25.130240
154.679760	4743.408248	25.135258
155.251291	4756.102604	25.140275
155.306781	4761.507373	25.145293
155.604885	4773.679563	25.150311
155.564492	4764.516294	25.155328
155.835936	4775.701520	25.160346
155.934379	4790.562782	25.165363
155.825649	4786.359617	25.170381
155.816457	4803.955508	25.175399
156.191883	4813.940775	25.180416
156.533576	4813.136049	25.185434
156.375338	4826.696035	25.190451
157.165243	4830.934647	25.195469
157.025062	4843.873139	25.200487
157.078228	4845.588325	25.205504
157.628260	4845.701071	25.210522
157.573205	4864.790927	25.215539
158.026771	4867.750187	25.220557
157.764959	4873.353056	25.225575
158.003523	4865.414956	25.230592
158.486598	4872.009067	25.235610
158.257026	4885.614994	25.240627
158.705065	4887.230443	25.245645
158.473315	4891.079891	25.250663
158.672333	4887.399822	25.255680
158.903354	4916.788858	25.260698
158.933165	4915.821500	25.265715
159.155019	4915.436424	25.270733
159.125054	4923.048419	25.275751
159.542256	4936.092203	25.280768
159.914984	4930.746668	25.285786
159.786010	4939.229602	25.290803
160.569665	4948.298723	25.295821
160.520109	4957.031216	25.300839
160.729277	4952.298415	25.305856
161.017354	4946.268543	25.310874
160.624457	4946.323838	25.315891
161.197989	4950.561655	25.320909
161.267708	4967.068962	25.325927
161.152189	4972.588968	25.330944
161.621841	4968.197296	25.335962
161.239897	4973.500205	25.340979
161.550106	4979.657425	25.345997
161.700181	4992.831483	25.351015
162.194273	4987.672094	25.356032
162.291402	4987.849482	25.361050
162.137621	5003.179722	25.366067
162.669830	5003.042738	25.371085
162.960122	5011.191715	25.376103
162.891803	5017.676557	25.381120
163.500167	5007.644486	25.386138
163.629392	5017.188641	25.391155
163.562643	5008.985813	25.396173
163.925603	5020.627178	25.401191
163.919550	5031.303640	25.406208
163.801111	5024.485159	25.411226
163.663560	5041.350129	25.416243
164.118636	5024.640701	25.421261
164.484602	5026.849827	25.426279
164.407817	5032.303808	25.431296
165.101936	5052.198206	25.436314
164.703413	5056.004371	25.441331
165.031588	5051.259214	25.446349
165.183543	5054.262601	25.451367
165.161465	5049.947947	25.456384
165.272839	5062.907160	25.461402
165.038456	5070.295559	25.466419
165.740553	5070.176152	25.471437
165.854549	5075.754929	25.476455
165.687102	5094.247104	25.481472
166.045857	5095.702950	25.486490
166.136884	5105.095307	25.491507
166.257067	5114.123252	25.496525
166.646479	5119.699931	25.501543
166.698935	5133.959460	25.506560
167.111954	5144.712380	25.511578
166.851152	5163.878975	25.516595
167.188486	5144.672093	25.521613
167.487594	5160.221918	25.526631
167.386882	5166.269967	25.531648
167.986219	5165.554283	25.536666
167.992096	5183.804748	25.541683
168.384350	5197.174600	25.546701
168.301710	5202.146592	25.551719
168.214217	5199.931808	25.556736
168.823176	5207.134480	25.561754
168.827547	5216.635168	25.566771
169.328589	5215.148892	25.571789
169.538193	5219.828892	25.576807
169.346005	5234.979105	25.581824
169.596557	5239.662164	25.586842
169.565302	5241.936704	25.591859
170.000001	5241.631914	25.596877
170.228431	5253.780620	25.601895
170.052484	5248.208448	25.606912
170.189227	5256.839297	25.611930
170.959720	5270.291993	25.616947
170.663552	5285.123939	25.621965
170.862268	5280.149634	25.626983
171.020246	5289.506345	25.632000
171.263434	5295.876195	25.637018
171.365996	5306.579994	25.642035
171.689704	5299.887851	25.647053
171.937754	5313.643389	25.652071
171.991950	5324.638870	25.657088
172.307569	5329.207591	25.662106
172.307188	5334.100443	25.667123
172.895988	5319.418433	25.672141
173.114243	5330.754382	25.677159
172.966196	5349.995048	25.682176
173.483415	5343.547198	25.687194
173.335631	5353.920922	25.692212
173.447526	5343.609751	25.697229
173.868413	5348.064130	25.702247
173.959281	5367.191627	25.707264
173.944809	5360.277817	25.712282
173.700796	5364.239767	25.717300
174.014659	5363.130031	25.722317
174.326822	5382.529066	25.727335
174.176777	5397.638090	25.732352
174.192686	5400.100970	25.737370
174.549208	5416.746837	25.742388
174.599535	5420.728975	25.747405
174.920354	5431.584895	25.752423
174.897198	5452.090849	25.757440
175.484607	5442.986716	25.762458
175.558644	5458.354250	25.767476
175.750582	5477.851138	25.772493
176.225224	5476.596255	25.777511
176.044905	5481.896132	25.782528
176.191030	5488.237064	25.787546
176.164841	5492.995110	25.792564
176.474420	5502.814301	25.797581
176.885208	5518.286962	25.802599
177.009372	5525.995014	25.807616
176.855215	5527.512310	25.812634
177.233130	5544.792583	25.817652
177.532546	5550.778074	25.822669
177.872572	5555.949104	25.827687
177.656093	5573.047896	25.832704
178.298003	5571.930948	25.837722
178.284485	5577.649808	25.842740
178.414464	5596.398934	25.847757
178.759537	5598.535645	25.852775
178.591282	5600.661233	25.857792
179.347992	5619.937214	25.862810
179.372088	5615.009115	25.867828
179.453820	5626.110946	25.872845
179.630695	5622.920324	25.877863
179.472600	5642.147089	25.882880
180.333241	5643.464377	25.887898
179.961740	5645.340868	25.892916
180.231194	5658.010580	25.897933
180.663385	5661.914007	25.902951
180.843843	5666.317745	25.907968
181.223587	5664.986174	25.912986
180.901480	5680.554849	25.918004
181.400208	5689.962554	25.923021
181.756818	5688.495712	25.928039
181.700127	5698.441837	25.933056
181.811221	5701.931546	25.938074
182.177182	5717.477689	25.943092
182.470086	5706.992749	25.948109
182.814511	5711.509704	25.953127
182.648067	5716.204551	25.958144
183.358284	5723.928202	25.963162
183.236594	5734.705264	25.968180
182.592343	5738.679489	25.973197
183.100074	5743.562296	25.978215
183.461193	5762.808860	25.983232
183.420221	5755.431863	25.988250
183.999868	5763.614765	25.993268
183.831435	5780.841960	25.998285
184.377462	5777.356728	26.003303
184.534601	5787.985969	26.008320
184.410727	5787.733956	26.013338
184.607191	5807.179980	26.018356
184.817065	5809.855594	26.023373
184.956550	5815.376941	26.028391
184.746724	5844.388288	26.033408
185.368954	5846.112276	26.038426
185.678430	5852.317259	26.043444
185.534873	5864.272114	26.048461
185.818497	5867.649596	26.053479
185.786149	5885.578454	26.058496
186.059782	5886.700464	26.063514
186.603194	5900.220772	26.068532
186.726371	5913.125076	26.073549
186.711882	5910.519963	26.078567
186.802361	5910.976193	26.083584
186.985334	5931.317810	26.088602
187.486750	5928.111016	26.093620
187.292410	5935.982780	26.098637
187.669923	5941.062817	26.103655
188.001241	5950.001280	26.108672
188.199775	5942.217351	26.113690
188.671853	5966.895230	26.118708
188.478764	5972.904353	26.123725
188.865955	5975.530116	26.128743
188.922984	5993.489272	26.133760
189.138928	5985.317478	26.138778
189.612904	6000.644911	26.143796
189.456024	6003.952533	26.148813
189.715448	6006.768779	26.153831
189.949830	6025.880796	26.158848
190.435788	6027.512509	26.163866
189.982076	6024.398509	26.168884
189.963399	6030.809641	26.173901
190.557286	6048.192297	26.178919
190.823167	6061.408963	26.183936
190.895959	6063.881962	26.188954
191.318976	6077.414950	26.193972
191.104111	6086.338029	26.198989
191.656164	6084.957339	26.204007
191.508670	6098.788063	26.209024
191.679732	6112.164830	26.214042
192.369852	6120.156966	26.219060
191.979853	6125.407801	26.224077
192.356401	6146.767371	26.229095
192.471482	6151.276171	26.234112
192.748714	6161.899443	26.239130
193.381771	6174.957653	26.244148
192.892165	6190.578255	26.249165
193.641219	6197.907744	26.254183
193.843041	6215.424587	26.259200
194.234828	6216.578616	26.264218
194.242589	6213.528028	26.269236
194.227486	6224.553848	26.274253
194.546794	6222.032139	26.279271
194.634915	6234.269772	26.284288
194.870337	6260.298335	26.289306
195.172151	6252.561230	26.294324
195.270863	6257.732385	26.299341
195.547980	6283.565043	26.304359
195.688840	6290.841482	26.309376
196.189545	6282.684924	26.314394
197.121663	6295.611138	26.319412
196.701383	6306.867791	26.324429
197.031657	6301.244402	26.329447
197.048824	6315.952331	26.334464
197.190698	6305.377067	26.339482
197.312638	6290.615897	26.344500
197.659998	6306.212808	26.349517
197.487087	6312.695553	26.354535
197.619480	6324.291800	26.359552
198.046387	6319.167822	26.364570
197.952768	6334.524476	26.369588
197.716993	6342.693329	26.374605
198.323145	6352.917939	26.379623
198.661200	6367.667185	26.384640
198.452616	6375.774971	26.389658
198.814093	6381.747858	26.394676
199.153174	6403.429275	26.399693
199.613472	6398.470511	26.404711
199.742412	6407.564018	26.409728
199.574712	6419.876577	26.414746
200.052625	6416.048337	26.419764
199.892695	6437.628033	26.424781
200.391875	6442.809109	26.429799
200.425887	6448.637597	26.434816
200.962651	6453.935903	26.439834
200.949550	6472.291645	26.444852
201.279367	6475.081153	26.449869
201.671964	6465.448283	26.454887
201.892966	6472.213466	26.459904
201.972671	6489.314063	26.464922
202.460106	6491.475931	26.469940
202.356289	6494.289180	26.474957
202.350396	6486.893766	26.479975
202.490669	6502.627461	26.484992
202.716889	6510.720856	26.490010
203.047394	6510.429217	26.495028
202.891698	6528.242285	26.500045
203.327791	6529.149477	26.505063
203.414488	6536.759651	26.510080
203.749779	6552.349192	26.515098
204.014938	6552.932758	26.520116
203.844408	6563.411746	26.525133
204.442325	6579.452632	26.530151
204.773370	6588.138905	26.535168
204.771619	6588.713776	26.540186
205.338645	6608.156266	26.545204
204.942999	6613.524926	26.550221
205.519736	6607.341958	26.555239
205.440833	6626.412135	26.560256
205.438862	6637.691848	26.565274
206.171284	6637.106796	26.570292
206.258048	6660.198110	26.575309
206.581931	6667.174539	26.580327
206.777376	6677.798297	26.585344
206.693237	6681.457681	26.590362
207.427366	6688.376163	26.595380
207.459014	6698.507872	26.600397
207.540340	6708.735980	26.605415
207.929518	6707.251331	26.610432
207.719767	6729.435818	26.615450
208.273465	6724.219259	26.620468
208.244321	6738.514921	26.625485
208.857572	6753.859051	26.630503
209.152370	6755.492368	26.635520
208.994484	6755.005748	26.640538
209.529921	6764.717631	26.645556
209.576544	6781.258606	26.650573
209.640179	6784.522351	26.655591
209.881019	6774.300665	26.660608
209.945514	6793.597942	26.665626
210.747539	6793.933255	26.670644
210.307382	6800.824233	26.675661
210.786342	6810.996419	26.680679
210.635871	6822.624666	26.685696
210.831405	6829.655991	26.690714
211.419743	6851.639833	26.695732
211.318419	6853.732980	26.700749
211.569375	6867.344018	26.705767
212.148960	6876.038846	26.710784
211.990791	6883.169798	26.715802
212.475122	6896.510690	26.720820
212.232191	6909.971837	26.725837
212.847506	6921.000334	26.730855
212.836799	6929.648759	26.735872
213.055969	6926.416561	26.740890
212.979822	6937.828041	26.745908
213.366456	6958.350405	26.750925
213.657844	6968.526808	26.755943
214.100577	6976.311841	26.760960
213.934493	6981.729880	26.765978
214.685550	6988.642670	26.770996
214.548618	7001.206505	26.776013
215.186950	7001.078149	26.781031
214.983948	7004.617314	26.786048
214.893496	7018.970152	26.791066
215.931835	7024.543623	26.796084
215.631119	7024.164607	26.801101
215.789616	7038.121731	26.806119
216.338304	7045.539780	26.811136
216.358338	7046.177548	26.816154
216.750849	7059.450864	26.821172
216.875218	7070.439557	26.826189
217.121900	7075.502526	26.831207
217.552063	7078.497391	26.836224
217.596732	7091.250665	26.841242
217.782270	7096.686263	26.846260
217.811716	7097.751898	26.851277
218.213278	7107.901648	26.856295
218.878706	7111.569968	26.861312
218.831978	7122.746499	26.866330
218.980190	7123.269482	26.871348
219.155881	7140.914423	26.876365
219.691365	7145.243960	26.881383
219.911950	7140.691911	26.886400
219.807205	7146.839108	26.891418
220.078163	7156.403218	26.896436
220.545366	7171.315983	26.901453
220.641685	7171.461952	26.906471
220.945584	7165.409936	26.911488
220.554034	7183.484728	26.916506
221.309392	7183.985208	26.921524
221.096470	7189.170719	26.926541
221.221652	7204.528550	26.931559
221.825758	7215.574767	26.936576
221.444522	7221.787402	26.941594
221.707700	7242.850318	26.946612
222.127697	7252.722608	26.951629
222.365274	7265.742535	26.956647
222.748556	7275.895243	26.961664
222.647416	7309.908254	26.966682
222.775416	7307.012281	26.971700
222.688974	7325.746570	26.976717
223.137522	7334.774683	26.981735
223.652946	7356.360151	26.986752
223.576952	7361.682107	26.991770
224.139284	7376.936872	26.996788
224.219980	7394.000273	27.001805
224.318936	7408.768874	27.006823
224.788112	7416.335279	27.011840
224.884115	7435.511486	27.016858
225.476576	7446.130319	27.021876
225.789734	7460.076163	27.026893
225.784883	7460.433716	27.031911
226.173885	7471.567455	27.036928
226.533326	7478.724886	27.041946
226.591284	7484.799352	27.046964
226.656066	7493.695088	27.051981
226.724483	7506.015580	27.056999
227.047434	7507.654027	27.062016
227.404341	7527.796534	27.067034
227.949701	7533.595771	27.072052
228.382172	7544.858495	27.077069
228.376069	7557.345388	27.082087
228.829536	7557.204951	27.087104
228.707749	7555.715045	27.092122
228.602374	7573.379176	27.097140
228.878796	7574.393520	27.102157
228.696398	7588.672810	27.107175
229.559669	7587.742066	27.112192
229.520626	7610.709061	27.117210
229.830334	7615.954883	27.122228
229.991873	7624.065217	27.127245
229.940929	7636.395024	27.132263
230.478200	7653.254545	27.137280
230.520467	7661.835032	27.142298
230.603468	7677.932291	27.147316
231.175133	7680.336828	27.152333
231.692049	7697.913063	27.157351
231.770266	7701.332537	27.162368
232.057222	7712.946489	27.167386
232.000245	7720.014556	27.172404
232.043287	7727.688888	27.177421
232.641015	7759.045533	27.182439
232.582863	7758.840021	27.187456
232.996639	7773.073414	27.192474
233.274207	7788.278421	27.197492
233.357285	7802.513131	27.202509
233.672663	7811.619168	27.207527
234.157078	7826.188810	27.212544
234.301299	7838.567105	27.217562
234.233341	7852.408784	27.222580
234.712265	7864.699936	27.227597
234.874433	7876.908121	27.232615
235.088949	7888.381994	27.237632
235.381956	7894.533427	27.242650
235.443084	7904.326534	27.247668
235.770829	7924.000486	27.252685
236.084865	7933.659278	27.257703
236.401966	7938.045316	27.262720
236.680645	7955.318157	27.267738
236.903329	7972.277766	27.272756
237.258617	7968.743085	27.277773
237.723532	7986.179361	27.282791
238.089582	7986.579846	27.287808
238.114932	8002.045536	27.292826
238.123589	8008.756153	27.297844
238.569593	8015.461402	27.302861
238.841080	8021.881443	27.307879
239.133208	8025.952551	27.312896
239.205677	8035.955475	27.317914
239.376588	8044.162395	27.322932
239.960430	8057.775838	27.327949
240.014398	8061.142351	27.332967
240.154760	8062.853651	27.337984
240.262058	8077.640424	27.343002
240.850415	8083.726710	27.348020
241.281402	8091.599301	27.353037
241.270827	8113.886846	27.358055
241.428332	8106.982946	27.363072
241.490010	8122.951336	27.368090
241.804705	8130.242315	27.373108
242.017028	8142.480705	27.378125
242.228751	8146.078244	27.383143
242.581793	8158.821833	27.388160
242.986789	8159.857112	27.393178
242.897933	8180.834180	27.398196
243.503884	8180.628812	27.403213
243.457468	8200.367988	27.408231
243.623624	8216.809442	27.413248
243.529904	8226.551207	27.418266
243.777961	8235.778500	27.423284
244.117192	8240.426341	27.428301
244.729149	8269.716881	27.433319
244.964040	8269.983222	27.438336
244.913552	8278.613254	27.443354
245.258072	8291.083602	27.448372
245.377821	8299.585948	27.453389
245.495327	8321.345383	27.458407
246.056422	8319.309599	27.463424
246.611465	8327.241785	27.468442
246.505620	8343.047181	27.473460
246.707970	8345.935876	27.478477
246.927919	8361.756550	27.483495
247.497407	8373.535029	27.488512
247.804774	8376.034736	27.493530
247.522467	8383.662438	27.498548
248.229073	8395.457337	27.503565
248.114774	8397.577947	27.508583
248.666852	8409.955875	27.513600
248.891343	8417.554712	27.518618
248.832990	8430.574465	27.523636
249.234751	8436.608015	27.528653
249.263497	8452.345063	27.533671
249.714063	8461.316588	27.538688
249.516698	8466.556846	27.543706
249.825082	8497.192889	27.548724
250.562933	8504.275656	27.553741
250.402621	8516.484268	27.558759
251.015616	8529.408392	27.563776
251.262327	8543.914812	27.568794
251.529497	8551.090274	27.573812
251.447563	8561.212385	27.578829
251.645203	8573.743819	27.583847
251.963489	8588.861022	27.588864
252.401508	8607.751238	27.593882
252.969688	8627.312503	27.598900
253.424263	8630.635306	27.603917
253.088422	8641.772802	27.608935
253.374896	8654.842880	27.613952
253.641364	8664.926255	27.618970
253.833949	8680.300013	27.623988
254.386189	8697.521223	27.629005
254.792304	8716.050314	27.634023
254.890509	8719.091141	27.639040
255.306507	8737.751308	27.644058
255.495242	8739.436151	27.649076
255.975478	8751.778205	27.654093
256.035315	8762.455983	27.659111
255.726182	8764.878675	27.664128
256.570183	8779.629532	27.669146
256.401170	8789.550719	27.674164
256.789198	8802.545006	27.679181
257.023585	8825.028666	27.684199
257.568022	8828.994127	27.689216
257.581476	8841.090486	27.694234
258.001679	8862.048566	27.699252
258.075248	8858.314747	27.704269
258.346874	8881.414611	27.709287
258.865160	8888.269875	27.714304
259.074491	8890.058851	27.719322
259.183438	8916.117296	27.724340
259.944560	8917.807207	27.729357
259.704429	8929.188773	27.734375
259.875202	8933.430641	27.739392
259.809309	8946.335119	27.744410
260.888900	8967.237382	27.749428
260.755957	8972.827614	27.754445
260.947326	8990.433981	27.759463
261.185459	8994.526392	27.764480
261.606480	9011.512715	27.769498
261.563912	9017.985458	27.774516
262.033640	9040.893470	27.779533
262.540898	9044.151266	27.784551
262.760625	9059.814710	27.789568
262.884399	9066.495048	27.794586
262.829528	9070.617590	27.799604
263.588308	9087.929942	27.804621
263.747993	9100.022507	27.809639
263.637542	9101.915272	27.814656
264.221117	9112.577508	27.819674
264.445367	9113.849537	27.824692
264.884381	9130.807893	27.829709
264.873180	9148.569276	27.834727
264.930940	9155.919856	27.839744
265.271270	9169.569112	27.844762
265.566283	9180.361838	27.849780
265.847463	9190.152727	27.854797
265.957585	9199.108483	27.859815
266.073531	9221.447000	27.864832
266.450287	9234.563333	27.869850
266.708187	9253.261416	27.874868
266.870683	9261.233399	27.879885
266.933361	9284.208634	27.884903
267.270408	9301.009469	27.889920
267.753423	9303.147116	27.894938
268.345560	9335.435556	27.899956
268.239276	9345.890267	27.904973
268.787906	9366.566744	27.909991
269.114319	9380.679301	27.915008
269.319811	9383.536094	27.920026
270.015592	9397.461353	27.925044
270.252463	9410.732331	27.930061
270.416744	9424.554589	27.935079
270.402137	9429.873837	27.940096
270.725742	9436.983971	27.945114
271.184964	9460.197249	27.950132
271.727849	9463.496899	27.955149
271.855269	9470.811432	27.960167
271.842600	9484.449914	27.965184
272.441646	9493.960686	27.970202
272.582319	9515.206407	27.975220
272.519186	9519.589243	27.980237
272.823371	9540.941987	27.985255
272.980343	9550.774625	27.990272
273.846694	9562.059022	27.995290
273.764783	9566.766857	28.000308
274.790657	9573.738618	28.005325
275.283537	9573.086829	28.010343
275.312576	9582.257541	28.015360
275.792539	9587.972959	28.020378
275.799474	9604.980491	28.025396
276.097568	9596.592169	28.030413
276.322433	9604.791331	28.035431
276.390899	9617.267930	28.040448
276.678859	9622.517734	28.045466
276.821392	9629.138504	28.050484
277.513020	9637.946547	28.055501
277.385850	9650.797966	28.060519
277.856364	9650.174937	28.065536
278.136952	9656.692001	28.070554
278.085727	9674.696957	28.075572
278.274674	9684.988787	28.080589
278.990535	9704.392293	28.085607
278.802954	9707.976913	28.090624
279.047198	9708.450199	28.095642
278.934117	9727.566812	28.100660
279.433559	9747.619950	28.105677
280.104633	9753.049735	28.110695
280.442984	9774.564736	28.115712
281.102085	9770.356969	28.120730
280.992496	9779.707363	28.125748
281.244186	9783.052688	28.130765
281.473555	9792.312102	28.135783
281.224025	9802.540076	28.140800
282.473506	9800.999360	28.145818
282.655092	9826.447803	28.150836
282.854356	9814.402840	28.155853
282.740293	9823.071964	28.160871
282.712160	9843.671985	28.165888
283.112379	9844.376588	28.170906
283.121407	9869.394301	28.175924
283.287977	9871.815234	28.180941
283.805723	9890.798464	28.185959
283.711397	9913.483333	28.190976
283.866894	9925.640239	28.195994
284.504086	9952.223606	28.201012
284.955434	9971.138384	28.206029
285.381466	9988.266901	28.211047
285.638621	10014.284724	28.216064
285.994759	10010.945289	28.221082
285.928175	10035.485671	28.226100
286.460160	10041.625646	28.231117
286.741481	10063.393036	28.236135
286.717568	10070.633631	28.241152
287.184837	10094.733676	28.246170
287.533724	10119.594290	28.251188
287.853267	10126.329593	28.256205
288.501522	10137.231728	28.261223
288.847538	10158.853325	28.266240
288.920684	10171.392712	28.271258
288.869068	10182.685519	28.276276
289.069734	10197.803515	28.281293
289.649937	10211.517000	28.286311
289.721947	10228.682252	28.291328
290.056386	10252.493879	28.296346
290.302568	10271.371638	28.301364
290.605803	10292.760126	28.306381
291.275878	10302.834845	28.311399
291.528792	10323.445045	28.316416
291.951153	10338.102170	28.321434
292.367677	10350.742602	28.326452
292.590984	10366.804427	28.331469
292.874154	10374.622215	28.336487
293.078005	10384.877366	28.341504
293.572225	10387.205993	28.346522
293.863886	10405.432641	28.351540
294.164665	10412.912994	28.356557
294.458888	10423.450812	28.361575
294.730173	10433.218648	28.366592
295.293864	10455.595860	28.371610
295.503430	10464.697680	28.376628
296.052677	10460.333309	28.381645
296.393053	10476.572654	28.386663
296.442859	10476.527018	28.391680
296.579661	10478.166480	28.396698
296.956840	10495.906197	28.401716
296.939478	10506.947551	28.406733
297.109970	10511.603455	28.411751
297.430423	10535.382902	28.416768
297.964124	10545.217045	28.421786
298.420440	10560.254241	28.426804
298.220592	10574.210173	28.431821
298.841862	10591.223409	28.436839
298.817124	10606.743317	28.441856
298.975003	10609.026777	28.446874
299.473860	10638.916603	28.451892
299.590035	10656.561585	28.456909
300.194564	10667.050933	28.461927
300.102201	10675.309732	28.466944
300.496675	10695.708718	28.471962
300.787637	10705.940927	28.476980
301.106707	10729.714523	28.481997
301.819568	10727.048472	28.487015
302.068804	10745.200001	28.492032
302.456419	10748.296867	28.497050
302.339558	10769.600148	28.502068
302.737551	10774.624645	28.507085
303.072393	10796.820246	28.512103
303.313254	10806.046790	28.517120
303.603697	10824.172996	28.522138
304.073991	10833.748833	28.527156
304.698453	10855.971759	28.532173
304.787605	10845.500054	28.537191
304.827846	10875.288434	28.542208
305.078404	10881.602234	28.547226
305.542528	10896.679526	28.552244
305.751417	10908.869758	28.557261
306.133685	10906.413347	28.562279
306.218151	10936.128586	28.567296
307.093192	10949.812220	28.572314
307.066165	10965.200165	28.577332
307.355997	10982.420399	28.582349
307.632757	10993.258087	28.587367
307.719313	11012.376315	28.592384
308.256819	11024.076242	28.597402
308.705415	11032.989332	28.602420
309.011593	11070.377703	28.607437
309.349097	11061.379456	28.612455
309.466963	11091.064449	28.617472
309.851329	11102.188473	28.622490
310.307174	11121.220546	28.627508
310.639175	11129.653047	28.632525
311.253677	11142.307211	28.637543
311.040351	11153.449109	28.642560
311.039800	11176.660767	28.647578
311.801730	11195.553398	28.652596
311.790396	11210.370717	28.657613
312.252070	11220.320702	28.662631
312.380518	11238.475843	28.667648
313.319313	11261.452047	28.672666
313.377891	11264.414243	28.677684
313.779165	11283.467661	28.682701
314.357908	11286.342063	28.687719
314.271301	11303.403684	28.692736
314.745457	11319.433350	28.697754
314.819067	11328.285332	28.702772
314.750943	11337.058477	28.707789
315.245591	11358.329787	28.712807
315.539009	11383.169196	28.717824
315.654242	11400.151923	28.722842
316.366805	11422.585916	28.727860
316.363655	11441.364978	28.732877
317.139578	11458.209529	28.737895
317.439584	11481.863918	28.742912
317.450619	11502.232276	28.747930
317.991628	11510.619579	28.752948
318.351961	11540.311508	28.757965
318.948804	11540.398057	28.762983
319.077610	11560.628038	28.768000
319.432069	11567.191039	28.773018
319.792851	11584.006003	28.778036
320.329549	11593.751817	28.783053
320.574915	11599.791956	28.788071
320.610767	11624.883596	28.793088
321.279158	11641.966195	28.798106
321.875942	11652.460471	28.803124
321.303917	11662.989430	28.808141
321.676807	11680.847778	28.813159
321.834351	11684.482914	28.818176
322.423876	11694.946774	28.823194
322.863891	11707.180263	28.828212
322.899834	11731.877320	28.833229
323.259294	11747.284306	28.838247
323.510784	11763.339758	28.843264
323.493604	11775.938576	28.848282
324.270863	11786.316240	28.853300
324.272613	11811.561883	28.858317
324.609711	11830.821688	28.863335
325.058807	11849.726093	28.868352
325.386306	11868.712720	28.873370
325.855354	11884.314219	28.878388
326.224754	11898.257748	28.883405
326.762629	11915.102108	28.888423
326.794755	11927.746985	28.893440
327.154597	11955.674478	28.898458
327.950448	11963.996803	28.903476
328.130125	11982.656192	28.908493
328.203519	11996.017772	28.913511
328.736978	12016.140648	28.918528
329.070266	12034.264471	28.923546
329.275859	12044.539206	28.928564
329.290869	12068.946314	28.933581
330.025228	12081.490766	28.938599
330.352599	12096.899908	28.943616
330.351925	12110.513161	28.948634
330.747009	12128.750548	28.953652
330.952623	12156.749865	28.958669
331.189798	12176.631968	28.963687
332.005720	12193.856165	28.968704
332.092991	12202.580108	28.973722
332.496894	12219.237314	28.978740
332.598228	12241.783824	28.983757
333.295901	12253.892049	28.988775
333.610052	12273.279056	28.993792
334.034784	12299.008548	28.998810
334.377375	12301.967471	29.003828
334.458945	12324.021402	29.008845
335.371067	12344.918973	29.013863
335.706686	12361.612264	29.018880
335.915357	12371.097246	29.023898
336.551233	12383.546804	29.028916
336.416666	12395.706542	29.033933
336.828925	12418.356133	29.038951
337.018176	12437.361832	29.043968
337.162172	12459.128254	29.048986
337.904303	12457.477361	29.054004
338.242083	12486.766959	29.059021
338.492722	12501.140055	29.064039
338.538993	12513.966263	29.069056
338.918067	12527.444544	29.074074
339.585920	12543.593333	29.079092
339.686979	12563.914000	29.084109
339.856257	12587.558680	29.089127
340.470345	12598.878131	29.094144
340.682058	12617.485763	29.099162
341.348033	12631.408642	29.104180
341.513905	12645.173032	29.109197
342.045051	12654.373961	29.114215
342.364040	12671.177499	29.119232
342.526313	12694.283418	29.124250
342.855003	12707.523407	29.129268
343.103256	12724.328599	29.134285
343.395888	12743.981563	29.139303
343.851312	12752.676513	29.144320
343.736322	12776.397537	29.149338
344.804549	12785.245982	29.154356
344.733879	12808.293792	29.159373
345.189422	12819.110846	29.164391
345.734177	12825.515008	29.169408
345.764386	12842.430249	29.174426
346.256738	12848.766838	29.179444
346.382303	12880.228175	29.184461
346.756557	12880.264343	29.189479
347.264256	12895.936419	29.194496
347.282370	12916.924142	29.199514
347.934117	12931.310525	29.204532
348.169564	12954.263194	29.209549
348.235330	12966.843497	29.214567
348.770269	12993.753520	29.219584
349.041508	13003.557441	29.224602
349.305634	13021.380416	29.229620
349.574494	13040.011091	29.234637
350.028502	13060.769640	29.239655
350.549625	13067.806012	29.244672
350.683285	13097.851696	29.249690
351.307936	13120.437282	29.254708
351.850502	13137.032527	29.259725
351.986256	13155.188371	29.264743
352.293214	13171.687920	29.269760
352.652272	13188.011951	29.274778
353.308791	13211.941094	29.279796
353.592167	13227.449634	29.284813
354.153395	13242.482024	29.289831
354.746502	13254.973599	29.294848
354.907325	13270.084521	29.299866
355.069967	13279.630855	29.304884
355.242093	13303.386513	29.309901
355.703427	13312.519753	29.314919
355.850570	13341.079470	29.319936
356.174766	13355.864863	29.324954
356.709838	13366.928728	29.329972
357.419980	13393.875036	29.334989
357.738187	13403.305484	29.340007
358.312757	13418.219079	29.345024
358.466430	13440.787243	29.350042
359.138605	13454.637129	29.355060
359.114747	13474.807810	29.360077
359.329989	13491.536748	29.365095
359.717304	13496.108904	29.370112
359.747533	13516.201682	29.375130
360.286726	13533.599935	29.380148
360.867839	13554.920189	29.385165
360.730561	13574.824523	29.390183
361.438360	13592.786966	29.395200
361.691510	13613.334419	29.400218
361.640103	13634.447514	29.405236
362.392581	13659.811722	29.410253
362.680715	13677.817877	29.415271
362.963378	13697.350232	29.420288
363.391817	13730.998261	29.425306
363.695294	13741.438596	29.430324
363.947221	13761.440061	29.435341
364.513165	13778.660658	29.440359
364.767755	13798.690168	29.445376
365.481124	13836.582371	29.450394
366.052346	13846.466063	29.455412
366.583388	13873.352684	29.460429
366.816824	13880.254416	29.465447
367.216838	13897.134778	29.470464
367.245156	13904.141284	29.475482
368.012080	13916.069201	29.480500
368.498433	13937.944758	29.485517
368.609351	13947.145828	29.490535
368.948433	13949.755018	29.495552
369.271285	13975.622760	29.500570
369.772854	13976.706419	29.505588
369.743196	13996.916460	29.510605
370.261419	14011.144575	29.515623
370.853318	14031.077281	29.520640
370.900408	14040.998962	29.525658
371.183860	14056.195519	29.530676
371.437833	14072.767315	29.535693
371.463598	14098.151200	29.540711
372.177390	14106.136791	29.545728
372.323679	14133.864098	29.550746
373.051930	14148.258377	29.555764
373.593437	14167.526446	29.560781
373.664418	14189.817906	29.565799
374.253101	14209.141790	29.570816
374.339319	14232.640469	29.575834
374.875182	14249.291430	29.580852
375.375210	14275.962412	29.585869
375.315376	14295.514292	29.590887
375.697637	14310.904011	29.595904
375.841581	14339.686799	29.600922
376.003160	14362.314823	29.605940
376.673695	14388.987678	29.610957
376.987975	14408.051565	29.615975
377.797401	14433.098391	29.620992
377.843392	14458.706975	29.626010
378.475197	14488.357856	29.631028
379.011295	14515.693053	29.636045
379.354741	14528.878318	29.641063
379.931448	14550.140377	29.646080
380.305821	14571.904721	29.651098
380.525000	14589.802532	29.656116
381.111119	14618.150130	29.661133
381.191579	14630.694493	29.666151
382.021849	14650.056780	29.671168
382.362631	14685.706726	29.676186
382.817202	14695.868107	29.681204
382.751292	14709.370273	29.686221
383.681600	14737.392532	29.691239
384.365907	14741.501590	29.696256
384.175996	14764.311476	29.701274
384.986543	14773.479153	29.706292
385.470093	14797.408971	29.711309
385.405057	14816.870611	29.716327
386.418104	14823.514767	29.721344
386.411090	14845.317055	29.726362
386.556879	14850.947478	29.731380
387.095098	14868.306053	29.736397
387.208706	14893.557226	29.741415
387.596766	14906.388360	29.746432
388.115059	14930.638200	29.751450
388.548927	14943.484292	29.756468
388.931259	14957.285934	29.761485
389.361857	14986.309038	29.766503
389.726165	15000.625169	29.771520
389.849419	15023.714767	29.776538
389.630228	15051.124825	29.781556
390.417636	15070.863771	29.786573
390.551495	15101.430540	29.791591
390.755954	15127.384715	29.796608
391.453705	15153.681706	29.801626
391.705662	15180.335963	29.806644
392.680297	15202.000687	29.811661
392.798259	15231.824803	29.816679
393.334758	15244.740295	29.821696
393.670970	15277.584353	29.826714
394.188998	15287.625571	29.831732
394.652594	15303.770817	29.836749
395.020438	15324.737996	29.841767
395.304455	15341.874683	29.846784
395.372151	15365.617688	29.851802
395.981063	15382.940393	29.856820
396.653946	15400.995296	29.861837
396.645280	15419.248562	29.866855
397.104176	15433.032240	29.871872
397.773548	15459.400423	29.876890
397.834147	15490.917309	29.881908
398.296824	15503.351843	29.886925
398.823476	15525.500846	29.891943
399.096907	15540.485391	29.896960
399.390040	15563.596406	29.901978
399.869239	15591.807442	29.906996
400.550525	15612.353157	29.912013
400.807901	15634.831874	29.917031
401.375528	15650.405250	29.922048
401.647515	15669.357006	29.927066
401.695508	15684.553843	29.932084
402.462088	15715.647840	29.937101
402.731039	15738.961831	29.942119
403.481266	15759.951709	29.947136
403.781604	15782.581789	29.952154
404.227000	15801.774975	29.957172
404.842711	15823.970383	29.962189
404.929929	15842.505921	29.967207
405.301784	15855.062295	29.972224
405.678702	15886.186021	29.977242
405.859334	15913.152517	29.982260
406.650489	15936.024896	29.987277
407.035956	15959.260895	29.992295
407.262290	15976.827252	29.997312
407.642424	16007.521129	30.002330
408.440454	16035.714463	30.007348
408.962635	16051.020503	30.012365
409.252273	16082.436158	30.017383
409.724562	16091.761688	30.022400
410.127440	16117.013381	30.027418
410.422432	16131.303317	30.032436
410.980720	16148.271428	30.037453
411.194505	16176.600701	30.042471
411.947291	16186.975160	30.047488
412.490809	16210.796285	30.052506
412.386407	16233.392382	30.057524
412.915090	16241.711085	30.062541
413.019180	16265.048380	30.067559
413.819981	16286.890014	30.072576
414.025178	16302.640713	30.077594
414.337049	16332.215075	30.082612
415.021637	16357.820925	30.087629
415.226690	16383.283987	30.092647
415.872919	16408.750624	30.097664
416.149352	16425.703119	30.102682
416.142145	16450.889987	30.107700
416.941045	16470.135860	30.112717
417.281984	16496.395834	30.117735
417.726779	16514.073755	30.122752
417.983790	16533.477215	30.127770
418.550831	16556.322270	30.132788
419.161842	16577.521204	30.137805
419.575305	16599.843946	30.142823
420.016591	16627.332831	30.147840
420.655582	16644.825688	30.152858
421.096502	16663.417163	30.157876
421.449792	16681.264338	30.162893
421.816739	16709.270346	30.167911
421.939095	16717.071734	30.172928
422.399588	16738.060691	30.177946
422.853563	16753.889658	30.182964
423.423440	16763.812986	30.187981
423.761204	16785.313949	30.192999
424.134864	16800.331158	30.198016
424.501001	16825.043110	30.203034
424.474276	16833.809141	30.208052
425.135129	16855.998675	30.213069
425.839480	16888.838364	30.218087
426.232071	16909.683376	30.223104
426.478638	16928.798284	30.228122
426.636141	16952.175424	30.233140
427.506746	16969.423834	30.238157
427.529926	17000.642674	30.243175
428.103986	17025.139119	30.248192
428.818800	17047.566791	30.253210
429.130595	17076.058916	30.258228
429.480632	17087.381353	30.263245
429.656061	17114.953638	30.268263
430.168300	17133.130097	30.273280
430.866133	17155.061497	30.278298
431.056572	17178.095783	30.283316
431.539408	17206.693972	30.288333
431.942351	17239.834158	30.293351
432.285112	17257.582442	30.298368
432.856668	17281.763744	30.303386
433.163202	17309.871688	30.308404
434.103191	17332.093857	30.313421
434.181117	17363.244694	30.318439
434.959353	17384.999514	30.323456
435.096113	17407.050670	30.328474
435.533895	17434.127475	30.333492
436.086500	17459.398540	30.338509
436.287939	17478.647407	30.343527
436.909898	17513.611042	30.348544
437.572886	17531.618968	30.353562
437.809020	17560.711169	30.358580
438.274029	17579.173409	30.363597
438.669486	17601.405373	30.368615
439.205760	17621.239987	30.373632
439.628497	17646.519004	30.378650
439.992708	17677.713949	30.383668
440.623974	17695.802805	30.388685
441.287132	17722.705731	30.393703
441.786191	17748.674156	30.398720
442.111511	17765.579109	30.403738
442.304141	17791.109149	30.408756
442.656786	17812.255153	30.413773
442.758175	17842.101701	30.418791
442.961336	17862.633115	30.423808
443.918451	17890.103020	30.428826
444.295505	17925.396362	30.433844
445.088505	17947.686487	30.438861
445.586660	17985.121536	30.443879
446.116558	18000.187859	30.448896
446.249421	18024.268234	30.453914
446.494805	18042.165158	30.458932
447.242144	18057.715500	30.463949
447.515415	18087.939823	30.468967
447.950571	18119.257035	30.473984
448.958752	18140.155416	30.479002
449.104675	18168.529829	30.484020
449.503496	18184.507597	30.489037
449.625899	18213.024745	30.494055
450.370572	18233.718118	30.499072
450.978027	18260.093526	30.504090
451.314516	18276.965590	30.509108
451.875924	18289.222210	30.514125
452.559878	18319.584730	30.519143
452.701837	18341.970967	30.524160
453.476185	18352.810727	30.529178
453.754392	18369.540378	30.534196
454.288184	18386.716466	30.539213
454.564723	18409.353357	30.544231
454.593718	18425.743036	30.549248
455.011932	18438.079038	30.554266
455.040937	18470.938753	30.559284
456.192264	18488.738414	30.564301
456.339067	18511.294663	30.569319
456.629085	18526.898062	30.574336
457.008732	18563.480956	30.579354
457.430430	18590.277603	30.584372
458.237580	18616.287383	30.589389
458.816703	18645.839220	30.594407
459.239682	18677.791008	30.599424
459.736168	18697.866713	30.604442
459.767670	18735.584786	30.609460
460.720248	18751.741630	30.614477
460.844081	18784.694422	30.619495
460.917597	18807.559426	30.624512
461.671343	18848.961545	30.629530
462.073583	18873.360890	30.634548
463.029608	18900.421750	30.639565
463.273999	18933.627574	30.644583
463.507961	18970.985867	30.649600
464.051803	18994.674548	30.654618
464.576671	19023.332014	30.659636
465.128043	19045.888693	30.664653
465.612406	19073.750217	30.669671
465.697775	19110.392868	30.674688
465.842129	19141.504563	30.679706
466.893371	19174.350660	30.684724
467.102332	19213.103258	30.689741
467.784682	19251.497482	30.694759
468.375677	19276.853356	30.699776
469.595970	19302.736167	30.704794
469.613616	19326.406583	30.709812
470.171097	19353.479955	30.714829
470.950113	19384.467359	30.719847
470.771712	19404.226201	30.724864
471.617017	19428.575799	30.729882
472.169707	19459.674587	30.734900
472.565960	19475.533779	30.739917
472.991661	19500.391445	30.744935
473.460257	19526.202754	30.749952
474.162154	19551.036178	30.754970
474.530659	19580.849872	30.759988
475.669835	19604.768266	30.765005
475.857510	19622.290286	30.770023
475.824534	19644.402156	30.775040
476.395530	19662.900324	30.780058
476.887333	19689.864409	30.785076
477.620795	19708.564622	30.790093
478.002863	19726.473278	30.795111
478.438899	19763.668759	30.800128
478.729702	19780.555601	30.805146
479.142113	19810.817668	30.810164
479.565696	19827.949112	30.815181
480.560671	19855.036792	30.820199
480.700370	19880.704224	30.825216
481.378091	19895.685687	30.830234
481.898592	19916.896143	30.835252
482.585484	19951.455959	30.840269
482.825696	19959.872001	30.845287
483.273242	19990.779607	30.850304
483.805619	20004.956248	30.855322
484.268753	20029.537046	30.860340
484.748147	20044.947730	30.865357
485.359645	20060.464097	30.870375
485.490143	20073.054701	30.875392
485.723273	20090.930156	30.880410
486.407286	20122.066295	30.885428
486.514165	20147.410673	30.890445
487.244243	20173.169246	30.895463
487.529971	20192.950959	30.900480
488.041172	20211.591696	30.905498
488.336552	20247.198993	30.910516
488.937787	20278.550528	30.915533
489.359379	20301.849263	30.920551
489.548864	20331.414139	30.925568
490.510014	20371.637091	30.930586
491.101244	20397.525117	30.935604
491.407838	20421.852925	30.940621
492.041877	20461.084785	30.945639
492.176019	20488.889455	30.950656
492.199174	20512.901628	30.955674
493.161122	20555.841691	30.960692
493.268093	20588.294700	30.965709
494.287564	20623.511261	30.970727
494.570644	20662.747948	30.975744
495.207957	20696.312232	30.980762
496.168502	20726.666775	30.985780
496.225835	20759.437439	30.990797
497.136926	20784.606132	30.995815
497.444535	20815.277903	31.000832
498.107375	20844.933691	31.005850
498.408241	20866.173258	31.010868
498.539266	20897.864803	31.015885
499.298044	20918.584100	31.020903
499.815505	20956.685260	31.025920
500.410481	21000.416711	31.030938
501.007329	21037.621014	31.035956
501.515972	21064.451667	31.040973
501.889581	21095.517919	31.045991
502.757742	21133.128519	31.051008
503.154195	21152.786444	31.056026
503.617765	21181.519860	31.061044
503.968321	21219.287517	31.066061
504.836658	21247.780715	31.071079
504.841366	21274.418887	31.076096
505.502693	21307.367558	31.081114
506.445198	21336.417936	31.086132
506.742852	21364.109772	31.091149
507.254035	21394.889570	31.096167
508.003977	21427.780333	31.101184
508.562187	21451.267547	31.106202
509.036890	21483.038894	31.111220
509.338222	21517.522850	31.116237
510.295723	21527.545879	31.121255
510.498042	21566.834928	31.126272
511.282626	21591.733816	31.131290
511.784770	21606.339701	31.136308
511.914247	21638.790914	31.141325
512.763610	21661.177565	31.146343
513.133047	21691.423987	31.151360
513.688718	21718.949537	31.156378
514.102368	21740.677876	31.161396
514.363587	21775.926806	31.166413
515.025291	21791.051244	31.171431
515.670059	21814.771764	31.176448
516.169126	21845.623669	31.181466
516.655988	21868.111564	31.186484
516.904206	21903.021546	31.191501
517.428687	21919.898905	31.196519
517.905965	21948.492281	31.201536
518.329427	21983.179077	31.206554
518.768824	22005.491318	31.211572
519.055178	22030.544622	31.216589
519.474255	22064.151739	31.221607
520.030543	22100.764119	31.226624
520.670257	22135.057141	31.231642
521.366339	22158.163433	31.236660
521.591970	22185.343241	31.241677
522.805851	22209.954516	31.246695
523.035436	22241.228375	31.251712
523.583939	22264.939239	31.256730
524.180098	22293.602958	31.261748
524.452728	22330.696192	31.266765
525.289161	22343.493625	31.271783
525.482832	22375.904398	31.276800
525.909217	22406.920217	31.281818
526.493841	22432.104241	31.286836
527.143948	22469.220758	31.291853
528.113164	22490.913460	31.296871
528.380668	22536.557364	31.301888
528.856848	22555.622860	31.306906
529.259522	22588.658414	31.311924
529.848286	22623.149831	31.316941
530.595986	22651.493344	31.321959
531.191259	22676.404297	31.326976
531.848657	22704.970556	31.331994
532.445471	22734.304623	31.337012
532.626141	22754.813089	31.342029
533.256691	22786.094517	31.347047
533.857566	22812.672981	31.352064
534.085587	22843.246625	31.357082
534.463409	22866.877519	31.362100
535.369783	22901.850474	31.367117
536.041090	22928.765609	31.372135
536.398642	22971.091548	31.377152
537.111443	23003.725354	31.382170
537.732942	23036.215536	31.387188
537.946028	23067.101499	31.392205
538.562956	23089.671517	31.397223
539.277416	23129.502722	31.402240
539.540800	23162.422027	31.407258
540.589853	23186.971871	31.412276
541.216908	23222.513628	31.417293
541.706699	23242.057907	31.422311
542.142353	23269.395880	31.427328
543.023692	23296.878939	31.432346
543.494638	23323.484756	31.437364
544.107361	23348.501247	31.442381
544.241072	23359.677948	31.447399
544.717670	23394.270423	31.452416
545.157310	23430.574931	31.457434
545.761051	23457.924753	31.462452
546.362297	23495.411038	31.467469
546.718789	23520.828072	31.472487
547.403988	23553.467105	31.477504
548.273912	23590.115264	31.482522
548.805158	23615.707266	31.487540
549.123449	23646.615566	31.492557
549.740781	23678.090048	31.497575
550.245966	23702.245446	31.502592
550.804509	23724.035419	31.507610
551.470078	23751.394919	31.512628
552.070333	23782.973351	31.517645
552.424298	23813.680423	31.522663
553.106036	23836.569745	31.527680
553.464623	23864.678927	31.532698
554.268572	23894.487814	31.537716
554.444913	23915.769115	31.542733
554.907364	23939.925176	31.547751
555.620912	23973.135520	31.552768
556.036432	23991.523084	31.557786
557.041057	24014.046071	31.562804
557.153170	24054.725476	31.567821
557.770316	24075.268052	31.572839
558.302197	24105.429517	31.577856
558.689428	24127.910302	31.582874
559.312328	24160.313630	31.587892
560.173532	24188.799548	31.592909
560.640230	24212.203259	31.597927
561.570903	24240.615177	31.602944
561.607127	24272.371194	31.607962
562.225577	24301.691547	31.612980
563.055773	24329.866549	31.617997
563.477499	24362.447061	31.623015
563.792369	24392.105790	31.628032
564.380836	24437.052868	31.633050
564.725139	24454.775825	31.638068
565.438679	24497.504255	31.643085
566.111272	24531.063197	31.648103
566.903794	24555.977211	31.653120
567.090052	24598.377667	31.658138
567.797156	24627.210644	31.663156
568.294715	24668.001555	31.668173
568.945839	24690.732344	31.673191
569.510021	24724.283311	31.678208
569.839436	24754.016133	31.683226
570.338968	24800.513625	31.688244
571.371159	24844.557931	31.693261
571.801853	24870.597027	31.698279
572.317133	24900.395751	31.703296
572.755412	24938.270490	31.708314
573.448269	24970.139640	31.713332
574.095742	25019.496248	31.718349
574.447031	25050.496344	31.723367
575.367256	25084.940110	31.728384
575.548929	25128.170286	31.733402
576.469043	25162.203419	31.738420
576.980332	25193.153398	31.743437
577.465833	25230.894898	31.748455
578.277680	25256.900080	31.753472
578.615653	25294.190820	31.758490
579.351137	25334.711991	31.763508
579.825915	25368.195880	31.768525
580.436934	25412.073562	31.773543
581.299551	25442.640271	31.778560
581.747783	25475.439634	31.783578
582.604436	25504.016617	31.788596
583.161875	25545.994387	31.793613
583.404955	25572.291292	31.798631
584.413051	25600.162148	31.803648
585.023945	25644.318432	31.808666
585.462188	25677.182887	31.813684
586.118801	25700.198358	31.818701
586.460879	25726.524200	31.823719
587.482958	25766.110245	31.828736
587.210204	25799.282171	31.833754
588.420997	25833.909234	31.838772
588.943023	25878.168428	31.843789
589.157481	25906.220885	31.848807
589.995927	25933.777495	31.853824
590.359859	25981.986393	31.858842
591.227163	26018.487732	31.863860
591.500846	26051.106809	31.868877
592.200810	26097.620148	31.873895
593.076669	26113.384266	31.878912
593.238098	26157.491987	31.883930
594.106001	26182.535260	31.888948
594.551630	26215.886082	31.893965
595.152521	26239.397543	31.898983
595.609169	26271.931441	31.904000
596.123834	26303.520928	31.909018
596.913410	26337.153049	31.914036
597.397523	26381.204400	31.919053
597.792354	26397.435927	31.924071
598.632698	26434.346731	31.929088
599.118670	26479.832679	31.934106
599.927715	26509.271771	31.939124
600.351738	26547.284491	31.944141
601.301878	26581.732457	31.949159
601.780516	26614.680596	31.954176
602.271480	26638.841760	31.959194
602.613481	26673.953946	31.964212
603.423262	26712.664989	31.969229
603.992722	26746.799963	31.974247
604.870388	26779.635315	31.979264
605.620415	26818.709853	31.984282
605.877888	26840.284915	31.989300
606.172259	26886.225242	31.994317
606.832096	26938.517226	31.999335
607.706773	26962.568120	32.004352
608.011690	27009.499364	32.009370
608.759623	27054.073371	32.014388
609.501717	27092.542927	32.019405
610.378764	27133.955673	32.024423
610.731639	27161.280310	32.029440
611.484973	27211.365185	32.034458
612.201042	27245.964709	32.039476
612.491506	27291.596866	32.044493
613.251729	27323.414945	32.049511
614.186072	27357.436919	32.054528
614.797923	27394.947780	32.059546
615.942327	27430.675101	32.064564
616.307132	27460.311560	32.069581
617.159771	27493.802999	32.074599
617.778338	27515.758340	32.079616
618.259807	27561.563445	32.084634
618.585254	27583.545804	32.089652
619.388879	27621.418920	32.094669
619.595559	27657.596886	32.099687
620.482709	27685.755031	32.104704
621.039211	27721.903608	32.109722
621.687456	27756.761127	32.114740
622.264494	27791.926925	32.119757
622.992483	27825.703897	32.124775
623.259560	27859.628956	32.129792
623.771256	27900.095510	32.134810
624.965931	27934.418994	32.139828
625.251784	27977.310263	32.144845
625.673899	28016.899870	32.149863
626.917004	28041.197736	32.154880
627.579934	28085.951657	32.159898
628.389708	28120.607524	32.164916
629.006314	28148.486327	32.169933
629.446220	28175.444739	32.174951
629.721372	28200.311555	32.179968
630.709877	28241.494200	32.184986
631.318848	28273.084627	32.190004
632.076940	28299.671015	32.195021
632.646314	28337.797056	32.200039
633.436875	28363.120615	32.205056
633.876030	28399.105469	32.210074
634.768980	28427.801000	32.215092
635.353326	28459.363969	32.220109
635.757812	28486.239847	32.225127
636.047728	28508.822924	32.230144
636.805032	28535.093703	32.235162
637.318721	28570.150670	32.240180
637.653854	28589.547386	32.245197
638.195450	28621.098337	32.250215
639.142940	28663.584029	32.255232
639.959514	28697.386499	32.260250
640.188575	28731.723496	32.265268
641.072631	28749.542674	32.270285
641.338899	28792.426080	32.275303
642.106050	28837.203251	32.280320
642.635169	28872.726066	32.285338
643.079390	28911.270995	32.290356
644.159871	28956.214268	32.295373
644.314563	28998.458202	32.300391
645.067014	29041.790626	32.305408
645.444113	29075.466598	32.310426
646.486644	29125.593059	32.315444
647.136982	29157.298473	32.320461
647.578934	29202.759472	32.325479
648.169916	29243.854692	32.330496
648.976250	29288.139995	32.335514
649.456512	29332.021343	32.340532
650.416691	29380.543137	32.345549
650.843810	29429.534113	32.350567
651.702978	29466.358979	32.355584
652.421722	29513.066818	32.360602
652.831933	29556.864801	32.365620
653.549780	29595.943385	32.370637
654.237664	29632.567814	32.375655
654.977502	29681.485131	32.380672
655.966495	29722.601152	32.385690
656.406292	29776.274953	32.390708
657.382052	29820.288344	32.395725
657.874575	29862.417933	32.400743
658.524383	29896.975440	32.405760
659.409038	29940.782114	32.410778
659.798266	29983.914241	32.415796
660.589651	30025.396841	32.420813
661.644578	30073.412376	32.425831
662.017723	30102.842754	32.430848
662.550277	30141.685901	32.435866
663.120237	30182.255300	32.440884
663.882351	30211.131856	32.445901
664.400533	30256.431533	32.450919
665.441542	30311.529693	32.455936
665.852785	30347.964829	32.460954
666.780585	30389.591155	32.465972
667.546947	30431.438810	32.470989
668.050212	30474.863852	32.476007
668.986261	30509.876950	32.481024
669.459675	30558.553612	32.486042
669.833960	30593.882400	32.491060
670.793287	30621.805718	32.496077
671.457254	30666.514534	32.501095
672.305737	30706.459772	32.506112
673.111828	30744.793428	32.511130
673.477335	30790.832514	32.516148
674.033757	30828.314094	32.521165
674.523983	30878.771540	32.526183
675.234527	30910.109901	32.531200
675.842963	30948.632927	32.536218
676.390537	30997.608763	32.541236
677.213543	31041.168246	32.546253
678.106858	31092.915904	32.551271
678.547941	31128.045495	32.556288
679.240885	31162.238035	32.561306
680.332097	31199.642858	32.566324
680.987871	31226.072059	32.571341
681.432937	31265.468356	32.576359
682.180263	31298.767576	32.581376
683.018782	31330.864097	32.586394
683.040256	31376.104937	32.591412
684.115274	31414.852880	32.596429
683.939276	31456.230663	32.601447
685.133802	31495.042222	32.606464
685.935079	31537.967661	32.611482
686.421547	31584.855643	32.616500
686.971490	31614.576572	32.621517
687.731813	31661.592526	32.626535
688.689862	31706.617873	32.631552
689.580180	31741.956310	32.636570
689.892187	31789.137588	32.641588
690.891558	31831.735488	32.646605
691.590033	31872.540947	32.651623
691.882738	31915.237042	32.656640
693.161469	31948.700637	32.661658
693.847166	32003.928487	32.666676
694.468009	32035.984327	32.671693
695.186836	32080.927833	32.676711
695.944558	32120.776218	32.681728
696.565265	32158.692667	32.686746
696.981397	32198.354463	32.691764
697.989710	32246.730049	32.696781
699.156031	32290.023445	32.701799
699.396320	32328.429670	32.706816
700.139830	32371.005525	32.711834
700.953291	32418.640745	32.716852
701.690989	32462.772906	32.721869
702.336647	32501.432067	32.726887
702.988092	32542.676102	32.731904
703.901672	32588.235051	32.736922
704.335243	32634.008355	32.741940
705.211781	32662.099122	32.746957
705.970862	32706.386502	32.751975
706.820910	32743.085871	32.756992
707.727502	32787.432509	32.762010
708.132658	32834.728006	32.767028
708.620588	32874.733881	32.772045
709.129109	32916.234955	32.777063
709.943866	32961.569953	32.782080
710.789542	33005.117358	32.787098
711.566770	33052.184381	32.792116
712.234473	33093.572367	32.797133
712.812578	33142.390412	32.802151
713.890764	33182.860795	32.807168
714.603321	33227.839365	32.812186
715.086607	33267.732919	32.817204
716.006668	33300.875526	32.822221
716.828181	33344.768824	32.827239
717.366731	33387.587482	32.832256
718.356409	33433.136357	32.837274
718.733524	33480.589438	32.842292
719.320998	33523.577738	32.847309
720.282564	33574.973147	32.852327
721.152902	33611.753054	32.857344
722.118488	33645.262097	32.862362
722.685907	33685.061078	32.867380
723.287847	33715.225746	32.872397
724.182815	33755.100013	32.877415
724.618322	33798.384537	32.882432
725.669423	33835.041693	32.887450
726.196560	33882.295160	32.892468
726.574877	33920.941908	32.897485
727.260873	33959.521577	32.902503
727.829573	34003.651840	32.907520
728.445474	34041.743162	32.912538
729.252092	34091.943865	32.917556
730.397528	34116.700462	32.922573
730.930068	34155.962062	32.927591
731.576296	34186.177374	32.932608
732.381789	34228.146660	32.937626
732.668265	34265.202500	32.942644
733.800920	34304.623301	32.947661
734.279645	34356.526170	32.952679
735.069873	34396.019735	32.957696
735.598601	34448.509322	32.962714
736.407521	34487.519614	32.967732
737.409708	34525.835838	32.972749
738.237751	34580.232570	32.977767
738.909484	34618.897876	32.982784
739.841714	34658.818604	32.987802
740.530750	34695.274732	32.992820
741.187066	34740.126247	32.997837
741.694140	34782.769317	33.002855
742.357511	34834.751932	33.007872
743.394383	34878.829681	33.012890
743.923847	34931.396226	33.017908
744.720326	34970.478910	33.022925
745.452692	35018.758686	33.027943
746.180553	35069.189023	33.032960
747.378906	35117.648963	33.037978
747.885843	35169.821292	33.042996
748.724920	35203.959621	33.048013
749.406712	35242.314674	33.053031
749.881535	35301.245144	33.058048
750.894225	35336.500936	33.063066
751.798806	35392.373646	33.068084
752.825103	35438.186687	33.073101
753.540486	35488.107822	33.078119
753.965704	35536.879482	33.083136
755.030171	35573.512281	33.088154
756.092063	35621.096889	33.093172
756.503110	35664.547140	33.098189
757.449435	35699.832900	33.103207
757.986411	35753.114803	33.108224
758.871279	35791.426404	33.113242
759.817952	35830.544064	33.118260
760.635596	35880.412170	33.123277
761.150766	35926.274693	33.128295
761.648164	35966.499937	33.133312
762.416391	36014.188321	33.138330
763.352807	36061.199197	33.143348
763.923822	36101.779907	33.148365
764.461655	36158.319082	33.153383
765.425676	36202.695537	33.158400
766.246020	36245.924804	33.163418
767.142436	36293.821374	33.168436
768.144748	36345.729323	33.173453
768.942964	36380.685312	33.178471
770.001498	36422.486541	33.183488
770.693079	36461.582078	33.188506
771.220194	36503.346543	33.193524
771.991951	36545.983323	33.198541
772.977840	36597.110378	33.203559
773.732698	36631.302134	33.208576
774.720649	36665.666111	33.213594
775.466702	36699.675981	33.218612
776.365534	36747.547901	33.223629
776.913190	36783.656686	33.228647
777.598194	36821.584105	33.233664
778.393076	36863.288374	33.238682
778.980319	36899.176163	33.243700
779.480700	36943.399126	33.248717
780.113235	36971.514885	33.253735
780.602375	37018.490420	33.258752
781.445449	37057.152308	33.263770
781.924150	37100.126963	33.268788
782.833088	37149.730810	33.273805
783.774703	37194.055929	33.278823
784.528510	37246.953499	33.283840
785.494342	37285.122319	33.288858
785.994153	37332.020990	33.293876
786.705984	37377.501723	33.298893
787.598404	37431.010388	33.303911
788.065063	37476.864869	33.308928
788.808953	37529.037487	33.313946
789.751196	37576.025497	33.318964
790.522800	37628.990782	33.323981
791.696493	37679.490283	33.328999
792.176560	37741.885658	33.334016
793.178812	37774.870643	33.339034
793.861948	37829.096022	33.344052
794.552531	37875.725710	33.349069
795.650802	37931.448273	33.354087
796.536745	37991.776226	33.359104
797.505766	38036.775427	33.364122
798.322124	38095.337619	33.369140
799.186998	38136.255595	33.374157
800.064676	38174.743343	33.379175
800.765208	38233.703471	33.384192
801.894393	38280.233738	33.389210
802.644802	38323.554042	33.394228
803.565448	38372.254589	33.399245
804.572424	38407.497391	33.404263
805.011497	38458.619663	33.409280
805.915047	38503.345524	33.414298
806.535125	38550.329201	33.419316
807.505100	38601.248523	33.424333
808.167793	38641.111423	33.429351
808.785551	38699.617823	33.434368
809.906115	38749.325030	33.439386
810.591101	38787.957879	33.444404
811.595319	38840.377488	33.449421
812.625480	38880.828326	33.454439
813.230448	38932.760498	33.459456
814.630967	38973.166162	33.464474
814.954572	39017.541230	33.469492
815.633671	39060.260759	33.474509
816.988210	39097.398046	33.479527
817.363558	39153.300215	33.484544
818.171056	39201.862255	33.489562
819.219033	39240.654090	33.494580
819.896278	39293.549709	33.499597
820.906869	39335.895349	33.504615
821.907313	39382.669499	33.509632
822.514715	39425.502162	33.514650
823.028815	39463.979582	33.519668
823.626928	39512.954552	33.524685
824.676067	39554.630555	33.529703
825.708794	39613.264171	33.534720
826.493763	39660.180171	33.539738
827.341037	39706.087302	33.544756
827.570674	39753.482561	33.549773
828.553281	39797.376582	33.554791
828.956481	39852.555236	33.559808
830.158073	39891.507586	33.564826
831.004219	39953.434627	33.569844
831.687643	40009.935831	33.574861
832.346899	40055.126882	33.579879
832.974702	40113.015751	33.584896
834.256644	40158.691344	33.589914
835.343787	40207.306712	33.594932
835.739534	40256.390938	33.599949
837.037137	40296.530601	33.604967
837.765364	40350.590812	33.609984
838.547406	40386.295797	33.615002
838.956408	40423.905966	33.620020
840.028263	40476.970354	33.625037
841.128034	40522.283128	33.630055
841.974079	40567.774863	33.635072
842.423527	40609.913614	33.640090
843.263607	40661.338776	33.645108
844.141251	40717.469886	33.650125
845.169855	40760.100086	33.655143
845.840622	40818.414165	33.660160
846.597152	40860.144819	33.665178
847.376819	40907.108612	33.670196
848.333447	40959.819074	33.675213
849.477296	41012.354883	33.680231
850.060809	41077.393639	33.685248
850.997564	41129.102020	33.690266
852.091901	41170.818319	33.695284
853.024822	41229.788148	33.700301
854.113731	41278.089401	33.705319
854.656922	41338.391795	33.710336
855.304096	41380.437823	33.715354
856.154468	41431.565930	33.720372
857.069939	41487.705745	33.725389
858.058349	41530.172979	33.730407
859.016939	41589.367446	33.735424
859.854218	41642.250035	33.740442
860.703119	41701.082497	33.745460
861.214778	41749.373984	33.750477
862.634689	41804.923320	33.755495
863.155113	41864.452780	33.760512
864.423517	41916.149036	33.765530
865.678418	41951.086812	33.770548
866.331480	42010.191111	33.775565
867.855075	42046.453125	33.780583
868.184617	42104.039778	33.785600
869.243438	42142.727569	33.790618
869.825061	42182.483155	33.795636
870.609402	42234.458355	33.800653
871.556767	42281.462085	33.805671
872.411704	42345.070622	33.810688
873.129978	42384.115759	33.815706
874.561723	42429.051608	33.820724
875.095914	42487.726733	33.825741
875.961304	42526.597288	33.830759
877.091686	42573.775385	33.835776
877.749520	42616.979584	33.840794
878.945499	42670.346105	33.845812
879.696985	42732.302158	33.850829
880.608808	42763.341811	33.855847
881.286159	42815.183335	33.860864
882.028474	42859.443713	33.865882
883.095463	42902.122674	33.870900
883.623677	42961.641230	33.875917
885.088162	43004.359349	33.880935
885.805888	43058.333005	33.885952
886.419583	43104.878406	33.890970
887.642223	43155.686577	33.895988
887.975197	43209.916928	33.901005
889.136137	43257.509165	33.906023
889.979209	43306.372037	33.911040
890.699427	43355.399734	33.916058
891.652866	43403.764825	33.921076
892.506726	43459.406975	33.926093
893.163129	43502.145062	33.931111
893.984805	43558.203641	33.936128
894.666654	43594.277428	33.941146
895.773905	43642.435523	33.946164
896.483268	43692.610542	33.951181
897.532656	43735.882124	33.956199
898.280512	43788.505552	33.961216
899.333575	43844.623504	33.966234
900.411221	43883.785806	33.971252
901.270755	43935.455944	33.976269
901.946890	43992.885713	33.981287
903.228902	44036.342846	33.986304
903.540181	44080.356889	33.991322
904.845332	44133.368278	33.996340
905.173859	44194.407882	34.001357
906.127072	44257.968578	34.006375
906.970063	44314.443209	34.011392
907.756483	44372.444958	34.016410
908.685231	44430.007089	34.021428
909.875884	44504.290995	34.026445
911.386297	44562.028062	34.031463
911.809237	44612.869910	34.036480
912.832549	44682.702120	34.041498
913.708840	44731.885533	34.046516
914.275120	44790.580701	34.051533
915.545197	44859.362728	34.056551
916.450607	44920.744134	34.061568
917.399860	44985.041298	34.066586
918.594859	45041.728331	34.071604
919.293558	45103.958619	34.076621
920.660316	45150.327132	34.081639
921.597833	45199.495663	34.086656
922.166126	45248.633555	34.091674
923.314388	45319.852506	34.096692
924.256181	45371.228435	34.101709
925.723913	45425.248543	34.106727
926.502140	45483.906018	34.111744
927.270412	45538.864602	34.116762
928.723996	45575.712703	34.121780
928.984382	45637.443780	34.126797
930.037134	45690.662866	34.131815
930.936429	45739.509624	34.136832
931.718610	45799.748775	34.141850
932.923054	45855.759523	34.146868
933.981260	45914.001057	34.151885
934.795867	45975.108578	34.156903
936.098894	46024.639203	34.161920
936.827844	46067.718775	34.166938
937.950861	46121.762911	34.171956
938.684999	46177.240807	34.176973
939.355167	46229.268528	34.181991
940.681002	46280.048696	34.187008
941.654155	46340.588349	34.192026
942.401188	46390.485183	34.197044
943.179277	46450.846914	34.202061
944.477915	46502.397298	34.207079
945.095335	46567.212761	34.212096
946.128416	46622.594338	34.217114
947.214488	46666.473166	34.222132
948.294683	46721.689457	34.227149
948.919745	46778.976215	34.232167
950.091406	46833.779911	34.237184
950.893130	46890.735634	34.242202
951.841660	46943.942376	34.247220
952.466904	47008.188519	34.252237
953.569815	47055.393066	34.257255
954.638444	47111.054958	34.262272
955.317486	47161.767579	34.267290
956.469253	47214.354792	34.272308
957.313005	47261.170159	34.277325
958.014377	47308.039548	34.282343
959.138406	47346.998214	34.287360
960.340858	47395.744162	34.292378
961.446418	47444.182743	34.297396
962.328634	47500.861693	34.302413
962.708239	47542.410864	34.307431
963.849363	47582.879264	34.312448
964.654358	47651.445319	34.317466
965.269939	47690.870098	34.322484
966.468247	47763.442796	34.327501
967.283923	47814.534051	34.332519
968.400506	47871.069681	34.337536
969.390243	47938.665033	34.342554
970.237649	47986.019078	34.347572
971.376722	48056.874854	34.352589
972.012204	48114.947846	34.357607
973.632061	48184.545680	34.362624
974.290301	48246.506277	34.367642
975.362617	48298.032929	34.372660
976.417092	48365.499208	34.377677
977.815087	48420.214367	34.382695
978.633371	48473.059168	34.387712
979.382471	48535.866749	34.392730
980.617866	48588.557936	34.397748
981.683387	48653.745740	34.402765
982.624376	48711.177709	34.407783
983.911808	48764.202797	34.412800
984.767009	48818.428170	34.417818
986.279743	48868.413027	34.422836
986.657194	48926.395626	34.427853
987.927933	48986.661662	34.432871
988.848335	49039.801800	34.437888
989.840250	49100.250982	34.442906
990.372325	49152.231108	34.447924
991.358924	49218.603343	34.452941
992.603156	49276.109464	34.457959
994.016196	49314.286013	34.462976
994.662971	49389.443032	34.467994
995.676952	49439.323752	34.473012
996.905771	49499.793839	34.478029
997.690495	49554.209145	34.483047
999.499132	49602.327125	34.488064
1000.152155	49665.026310	34.493082
1001.460058	49710.420072	34.498100
1002.389399	49768.147561	34.503117
1003.561436	49819.851846	34.508135
1004.978922	49852.302658	34.513152
1005.236882	49923.409742	34.518170
1006.277343	49961.247105	34.523188
1007.195096	50020.293068	34.528205
1008.142164	50073.121402	34.533223
1009.403949	50119.794939	34.538240
1009.904632	50181.405817	34.543258
1011.150972	50234.080104	34.548276
1011.902148	50288.268298	34.553293
1012.737171	50349.599502	34.558311
1014.098409	50394.593985	34.563328
1014.624557	50465.439300	34.568346
1015.835268	50513.399724	34.573364
1017.334920	50575.431023	34.578381
1017.963432	50642.173472	34.583399
1019.271476	50693.111814	34.588416
1019.843373	50755.396418	34.593434
1020.985721	50806.981027	34.598452
1022.243640	50872.296867	34.603469
1022.675717	50922.126386	34.608487
1023.730511	50971.010654	34.613504
1024.799508	51033.167557	34.618522
1025.725244	51079.003500	34.623540
1027.054013	51128.977803	34.628557
1027.457130	51183.912278	34.633575
1028.562633	51243.552061	34.638592
1029.523909	51303.834666	34.643610
1030.682118	51360.328101	34.648628
1031.758162	51421.358663	34.653645
1032.164674	51469.953184	34.658663
1033.698891	51530.557960	34.663680
1034.857684	51588.513507	34.668698
1036.060085	51646.905298	34.673716
1037.291839	51710.190143	34.678733
1037.601241	51771.733964	34.683751
1039.240316	51828.064667	34.688768
1040.072226	51904.023467	34.693786
1041.290467	51960.445691	34.698804
1042.138913	52015.382012	34.703821
1043.454772	52082.811944	34.708839
1044.542732	52141.634193	34.713856
1045.246093	52202.358154	34.718874
1046.700453	52254.042672	34.723892
1047.758450	52316.976715	34.728909
1048.640865	52375.781116	34.733927
1049.829320	52448.920664	34.738944
1051.134162	52507.558016	34.743962
1051.896461	52573.759868	34.748980
1052.917094	52626.841952	34.753997
1054.108865	52698.127725	34.759015
1055.558762	52752.857719	34.764032
1056.347940	52820.334280	34.769050
1057.780511	52875.377338	34.774068
1058.854102	52928.730242	34.779085
1059.695119	52986.220140	34.784103
1061.496924	53035.846063	34.789120
1062.302827	53095.702029	34.794138
1063.475427	53141.857753	34.799156
1064.176443	53190.226241	34.804173
1065.397572	53258.794449	34.809191
1066.574402	53314.144355	34.814208
1067.695829	53374.185768	34.819226
1068.365823	53431.349169	34.824244
1069.924263	53489.632884	34.829261
1070.604576	53542.074248	34.834279
1071.373921	53593.482975	34.839296
1072.913450	53663.856633	34.844314
1073.699494	53724.426055	34.849332
1074.895843	53773.926857	34.854349
1075.870203	53839.016983	34.859367
1076.983750	53889.144818	34.864384
1077.837868	53951.963305	34.869402
1079.224263	54014.167061	34.874420
1080.490373	54070.314778	34.879437
1081.530679	54134.199373	34.884455
1082.673109	54188.506252	34.889472
1083.309652	54240.057421	34.894490
1084.315853	54308.586406	34.899508
1085.892822	54366.597285	34.904525
1086.414559	54429.057747	34.909543
1088.093604	54491.792820	34.914560
1088.867622	54553.764807	34.919578
1089.849250	54615.634842	34.924596
1091.043197	54673.149552	34.929613
1092.356883	54727.120772	34.934631
1093.514789	54784.122472	34.939648
1094.387505	54846.851835	34.944666
1095.591508	54901.929106	34.949684
1096.465921	54962.139812	34.954701
1097.400477	55006.931566	34.959719
1098.507629	55046.893109	34.964736
1099.303018	55099.300935	34.969754
1100.391759	55164.933715	34.974772
1101.566111	55212.776602	34.979789
1102.365179	55276.759014	34.984807
1103.284862	55327.717648	34.989824
1104.344816	55394.671899	34.994842
1105.263833	55458.585393	34.999860
1106.857532	55509.692036	35.004877
1108.048848	55589.011237	35.009895
1109.267221	55647.321892	35.014912
1110.144901	55712.729759	35.019930
1111.246580	55776.248452	35.024948
1112.525186	55836.189252	35.029965
1113.440250	55905.939569	35.034983
1114.696358	55962.770515	35.040000
1115.699804	56029.406310	35.045018
1116.729115	56104.493389	35.050036
1118.445514	56160.094591	35.055053
1119.170047	56220.287651	35.060071
1120.847912	56292.400541	35.065088
1121.756737	56349.350067	35.070106
1122.908637	56410.552590	35.075124
1123.923017	56477.327159	35.080141
1125.411429	56541.179732	35.085159
1126.492873	56603.653216	35.090176
1127.752923	56662.225643	35.095194
1129.147903	56724.745291	35.100212
1130.438139	56787.452380	35.105229
1131.330388	56838.532464	35.110247
1132.410725	56895.551375	35.115264
1133.539783	56957.005702	35.120282
1134.356044	57019.110407	35.125300
1135.592584	57089.560668	35.130317
1137.036508	57155.744579	35.135335
1138.402940	57211.877699	35.140352
1139.187945	57279.367619	35.145370
1140.869290	57334.983379	35.150388
1141.997338	57387.382131	35.155405
1143.428453	57456.068850	35.160423
1144.402625	57511.061560	35.165440
1145.734640	57566.498372	35.170458
1146.146864	57636.408407	35.175476
1147.386373	57690.328343	35.180493
1148.643781	57742.853189	35.185511
1149.469674	57813.762271	35.190528
1150.989707	57867.638688	35.195546
1152.044595	57932.790703	35.200564
1153.478272	57989.193598	35.205581
1154.459143	58064.851375	35.210599
1155.185156	58122.359058	35.215616
1156.324720	58180.264171	35.220634
1157.377623	58241.278001	35.225652
1158.909535	58314.508464	35.230669
1160.246967	58384.244173	35.235687
1161.162073	58440.184990	35.240704
1162.020980	58502.780535	35.245722
1163.191502	58573.650555	35.250740
1164.567935	58638.526279	35.255757
1165.625058	58705.376301	35.260775
1166.967689	58771.257717	35.265792
1168.471639	58828.341480	35.270810
1169.534970	58890.127505	35.275828
1170.546063	58946.776022	35.280845
1172.032329	59008.331571	35.285863
1172.863706	59063.748933	35.290880
1174.193401	59106.593988	35.295898
1175.412468	59169.514642	35.300916
1176.586062	59208.611929	35.305933
1177.344316	59258.983900	35.310951
1178.925202	59302.941954	35.315968
1179.663103	59352.336225	35.320986
1180.928270	59415.560449	35.326004
1181.923071	59462.351250	35.331021
1182.666955	59518.720127	35.336039
1184.187338	59572.416737	35.341056
1185.065916	59638.012370	35.346074
1186.692537	59706.706533	35.351092
1187.971203	59767.100206	35.356109
1188.953495	59841.560670	35.361127
1190.295132	59897.716582	35.366144
1191.821752	59945.507434	35.371162
1192.673291	60017.096227	35.376180
1193.938260	60064.978914	35.381197
1195.223307	60124.315407	35.386215
1196.267233	60179.632410	35.391232
1197.446993	60236.314496	35.396250
1198.390204	60309.921657	35.401268
1200.010152	60371.117923	35.406285
1201.254599	60433.911278	35.411303
1202.414902	60504.630283	35.416320
1203.758473	60564.414435	35.421338
1205.078059	60633.488431	35.426356
1206.149798	60684.453590	35.431373
1207.279006	60753.785606	35.436391
1208.531412	60820.534906	35.441408
1210.326936	60869.576782	35.446426
1211.425377	60939.002758	35.451444
1212.489286	60991.507964	35.456461
1213.572151	61054.271237	35.461479
1214.746590	61125.249351	35.466496
1216.137691	61184.742726	35.471514
1217.370841	61250.128925	35.476532
1218.835516	61316.453883	35.481549
1219.833769	61378.231079	35.486567
1221.027233	61432.305797	35.491584
1222.807600	61495.980151	35.496602
1223.793327	61562.209837	35.501620
1224.933653	61621.984075	35.506637
1226.075914	61682.201266	35.511655
1227.508346	61742.620056	35.516672
1228.699197	61809.324709	35.521690
1229.561710	61869.617803	35.526708
1230.902355	61925.310087	35.531725
1232.107019	61999.691650	35.536743
1233.428450	62066.325914	35.541760
1234.874765	62119.729534	35.546778
1236.173160	62181.727630	35.551796
1237.224295	62235.541530	35.556813
1238.293376	62307.660007	35.561831
1239.343961	62371.197657	35.566848
1241.175496	62425.332925	35.571866
1242.156654	62499.599053	35.576884
1243.796580	62549.092779	35.581901
1244.798222	62618.114503	35.586919
1245.760469	62683.363329	35.591936
1247.305578	62734.182665	35.596954
1248.679133	62803.862023	35.601972
1249.802861	62853.690385	35.606989
1251.081372	62919.099227	35.612007
1252.002397	62978.259038	35.617024
1253.538532	63044.115327	35.622042
1255.006306	63103.500041	35.627060
1256.345322	63159.359954	35.632077
1257.495014	63210.248498	35.637095
1258.421366	63265.698459	35.642112
1259.525065	63296.342925	35.647130
1260.674501	63361.114758	35.652148
1261.647963	63410.543613	35.657165
1262.849966	63462.247461	35.662183
1263.972272	63521.104838	35.667200
1265.142696	63580.511918	35.672218
1266.558765	63647.566102	35.677236
1267.659875	63701.546287	35.682253
1269.102144	63764.412111	35.687271
1269.954459	63837.290659	35.692288
1271.672602	63893.833565	35.697306
1272.612370	63966.888723	35.702324
1274.031284	64039.976711	35.707341
1275.221794	64103.636160	35.712359
1276.319224	64180.130193	35.717376
1277.698932	64243.937644	35.722394
1278.978755	64318.276395	35.727412
1280.983260	64385.949500	35.732429
1281.937620	64452.710933	35.737447
1283.276220	64514.936465	35.742464
1284.879740	64580.722958	35.747482
1286.266583	64656.191850	35.752500
1287.461941	64711.596579	35.757517
1288.558505	64777.057768	35.762535
1290.005187	64850.764207	35.767552
1291.459784	64909.522186	35.772570
1292.931145	64975.210114	35.777588
1293.844761	65043.138067	35.782605
1295.486559	65112.553962	35.787623
1296.831838	65175.375202	35.792640
1298.408974	65236.938411	35.797658
1299.361274	65306.272843	35.802676
1300.674134	65381.502251	35.807693
1302.276919	65442.162931	35.812711
1303.244249	65509.437959	35.817728
1304.543737	65561.991917	35.822746
1306.030439	65641.075875	35.827764
1307.055840	65700.225777	35.832781
1308.670762	65767.691353	35.837799
1309.800593	65846.015093	35.842816
1311.878688	65903.949704	35.847834
1313.080160	65966.371235	35.852852
1314.095588	66026.181909	35.857869
1315.480215	66084.130520	35.862887
1316.699430	66149.398796	35.867904
1318.273232	66215.802019	35.872922
1319.794021	66271.665740	35.877940
1321.425861	66343.365856	35.882957
1322.512837	66406.445860	35.887975
1323.888788	66457.343561	35.892992
1325.071122	66513.013873	35.898010
1326.515872	66568.757195	35.903028
1327.807939	66626.569583	35.908045
1329.504268	66674.834358	35.913063
1330.154331	66739.294185	35.918080
1331.363555	66802.356036	35.923098
1332.960690	66861.482466	35.928116
1334.546566	66917.337423	35.933133
1335.723859	66980.208439	35.938151
1337.349016	67042.306705	35.943168
1338.322912	67107.128319	35.948186
1339.636981	67160.246819	35.953204
1340.817584	67217.419519	35.958221
1342.165281	67278.181516	35.963239
1343.073687	67351.833875	35.968256
1344.947731	67409.810207	35.973274
1345.717004	67464.002350	35.978292
1346.722836	67515.377994	35.983309
1348.544368	67573.027342	35.988327
1349.441785	67629.130925	35.993344
1350.727686	67678.063360	35.998362
1351.793641	67743.499014	36.003380
1353.093471	67810.645773	36.008397
1354.639075	67862.171895	36.013415
1355.541824	67936.928541	36.018432
1356.847474	67998.939853	36.023450
1358.286765	68076.829446	36.028468
1359.834696	68152.612781	36.033485
1361.300269	68219.722005	36.038503
1362.466145	68292.842887	36.043520
1364.076439	68366.179343	36.048538
1365.610272	68430.232820	36.053556
1366.465301	68509.304259	36.058573
1368.118926	68570.920563	36.063591
1369.576169	68650.512362	36.068608
1371.206614	68716.368687	36.073626
1372.745021	68793.333141	36.078644
1374.194746	68856.185114	36.083661
1375.576748	68927.551677	36.088679
1376.939183	69000.631137	36.093696
1378.375633	69072.021237	36.098714
1379.521644	69148.497289	36.103732
1381.081038	69212.023154	36.108749
1382.735065	69283.411441	36.113767
1384.214124	69356.169714	36.118784
1385.788190	69424.423866	36.123802
1387.325498	69483.160462	36.128820
1388.396399	69545.991096	36.133837
1390.121371	69619.788079	36.138855
1391.143079	69694.100613	36.143872
1392.687917	69749.480591	36.148890
1393.802527	69832.118450	36.153908
1394.816538	69906.369474	36.158925
1396.806161	69972.609704	36.163943
1398.359417	70058.155767	36.168960
1399.472669	70133.677353	36.173978
1400.783581	70191.779774	36.178996
1402.401934	70272.871094	36.184013
1404.075141	70339.402417	36.189031
1405.317134	70411.016615	36.194048
1406.687806	70482.674192	36.199066
1407.598972	70560.888236	36.204084
1409.196862	70632.662635	36.209101
1410.995058	70703.278711	36.214119
1412.395710	70781.771413	36.219136
1413.811828	70847.863014	36.224154
1415.632540	70912.700950	36.229172
1416.962312	70993.130448	36.234189
1418.401271	71058.370455	36.239207
1419.949618	71126.531786	36.244224
1421.251990	71200.697032	36.249242
1422.783623	71259.717163	36.254260
1424.335700	71334.261650	36.259277
1425.490114	71385.007468	36.264295
1426.759907	71464.573909	36.269312
1428.228970	71529.151790	36.274330
1429.677747	71599.027074	36.279348
1431.066608	71663.060567	36.284365
1432.804765	71734.486741	36.289383
1434.259789	71789.353174	36.294400
1435.583794	71864.783445	36.299418
1437.079261	71925.330583	36.304436
1438.471377	71989.415025	36.309453
1439.959966	72044.390726	36.314471
1441.095680	72097.851258	36.319488
1442.290679	72160.181138	36.324506
1443.888401	72226.399777	36.329524
1444.822196	72272.622251	36.334541
1446.006531	72328.342776	36.339559
1447.327867	72401.520529	36.344576
1448.586540	72466.589608	36.349594
1450.026722	72543.194210	36.354612
1451.743038	72607.837365	36.359629
1453.011324	72674.400006	36.364647
1454.298921	72758.324591	36.369664
1455.835507	72829.050670	36.374682
1457.322532	72908.080836	36.379700
1458.744822	72982.282997	36.384717
1460.272818	73056.050844	36.389735
1462.159712	73132.751890	36.394752
1463.502729	73209.284968	36.399770
1464.837082	73279.917246	36.404788
1466.226372	73358.660069	36.409805
1468.383036	73431.101950	36.414823
1470.187318	73505.701766	36.419840
1471.628412	73576.064802	36.424858
1473.076343	73638.371242	36.429876
1474.628620	73715.468337	36.434893
1476.090941	73780.470769	36.439911
1477.450467	73856.901798	36.444928
1479.193242	73930.245802	36.449946
1480.883045	73989.437283	36.454964
1481.845780	74075.012839	36.459981
1483.437800	74137.348561	36.464999
1485.101149	74211.630422	36.470016
1486.190165	74284.089741	36.475034
1488.052598	74343.900983	36.480052
1489.705378	74422.605711	36.485069
1491.347457	74499.488352	36.490087
1493.140264	74569.469629	36.495104
1494.851680	74623.567143	36.500122
1496.236888	74696.259886	36.505140
1497.505017	74767.590475	36.510157
1498.825604	74836.937027	36.515175
1500.289061	74900.029325	36.520192
1501.806599	74975.552145	36.525210
1502.883352	75042.581360	36.530228
1504.380055	75125.365983	36.535245
1506.298155	75201.219417	36.540263
1507.777582	75273.392299	36.545280
1509.146827	75347.622010	36.550298
1510.730857	75423.363688	36.555316
1512.048340	75503.403442	36.560333
1513.602532	75579.010890	36.565351
1515.378560	75655.394528	36.570368
1516.463532	75736.282064	36.575386
1518.092507	75807.090245	36.580404
1519.615357	75885.186236	36.585421
1521.272752	75967.251596	36.590439
1522.714314	76033.554810	36.595456
1524.508487	76123.769673	36.600474
1526.058907	76191.183633	36.605492
1527.617028	76260.015309	36.610509
1529.190040	76333.544464	36.615527
1530.707553	76411.288121	36.620544
1532.441126	76485.463937	36.625562
1534.028643	76545.133100	36.630580
1535.283137	76630.012396	36.635597
1536.635375	76695.571155	36.640615
1538.457020	76767.276434	36.645632
1539.961511	76841.919782	36.650650
1541.137029	76895.751046	36.655668
1543.246333	76969.362669	36.660685
1544.478228	77025.478234	36.665703
1545.629194	77077.641552	36.670720
1546.899794	77139.071781	36.675738
1548.636289	77205.965095	36.680756
1549.968684	77264.877695	36.685773
1551.478881	77337.760671	36.690791
1552.711688	77399.045386	36.695808
1553.920691	77483.402408	36.700826
1555.930631	77553.572797	36.705844
1557.235093	77626.235384	36.710861
1558.496634	77707.658549	36.715879
1560.216386	77788.427504	36.720896
1561.971134	77871.598177	36.725914
1564.273327	77952.289126	36.730932
1565.280660	78025.315982	36.735949
1566.744120	78093.698389	36.740967
1568.357684	78185.823263	36.745984
1569.841269	78265.262408	36.751002
1571.582025	78333.082608	36.756020
1573.095942	78420.397204	36.761037
1574.694569	78519.670541	36.766055
1576.691256	78595.660516	36.771072
1578.344169	78682.916186	36.776090
1579.796968	78758.599012	36.781108
1581.293658	78837.847732	36.786125
1582.846253	78925.930665	36.791143
1584.624352	79010.190639	36.796160
1586.382478	79084.889088	36.801178
1588.312427	79159.320142	36.806196
1589.501773	79245.522624	36.811213
1591.148242	79338.989102	36.816231
1592.867942	79428.618424	36.821248
1594.474255	79506.813056	36.826266
1596.304287	79584.352115	36.831284
1597.445547	79675.491694	36.836301
1598.846308	79750.412571	36.841319
1600.709868	79836.802759	36.846336
1602.205811	79921.743126	36.851354
1604.025329	80020.024425	36.856372
1605.917013	80098.087378	36.861389
1607.779986	80173.291794	36.866407
1609.267161	80251.747888	36.871424
1611.197403	80334.657807	36.876442
1612.600643	80406.539429	36.881460
1614.253958	80499.628663	36.886477
1616.014691	80582.135089	36.891495
1617.500673	80658.362696	36.896512
1619.458610	80739.039658	36.901530
1620.825099	80810.864727	36.906548
1622.590795	80893.041888	36.911565
1623.911173	80972.679047	36.916583
1625.596284	81055.363412	36.921600
1627.496747	81127.916583	36.926618
1629.219265	81206.085134	36.931636
1630.700978	81278.982968	36.936653
1632.452788	81352.484878	36.941671
1634.297916	81427.252027	36.946688
1635.782939	81506.535521	36.951706
1637.389903	81587.143161	36.956724
1639.311272	81664.648377	36.961741
1640.843571	81739.085220	36.966759
1642.561372	81803.217871	36.971776
1644.273132	81882.479610	36.976794
1645.657288	81944.738960	36.981812
1647.244045	82021.537326	36.986829
1648.547889	82111.734482	36.991847
1650.060868	82162.900470	36.996864
1651.381468	82244.619104	37.001882
1652.850847	82310.628967	37.006900
1654.517138	82385.337963	37.011917
1655.695503	82446.908425	37.016935
1657.455053	82510.542014	37.021952
1658.832390	82594.381391	37.026970
1660.675595	82672.623823	37.031988
1662.125650	82746.822791	37.037005
1664.136380	82832.261578	37.042023
1665.635740	82902.715458	37.047040
1667.293635	82995.292752	37.052058
1668.980660	83074.891143	37.057076
1670.743664	83154.262467	37.062093
1672.321927	83241.987524	37.067111
1674.071505	83323.705488	37.072128
1675.720185	83415.892804	37.077146
1677.455238	83490.087125	37.082164
1679.296623	83587.832633	37.087181
1680.653605	83668.726076	37.092199
1682.958943	83745.023861	37.097216
1684.292265	83839.238553	37.102234
1686.064009	83928.988130	37.107252
1688.330767	84008.435049	37.112269
1689.716530	84102.579048	37.117287
1691.727186	84175.363552	37.122304
1693.045765	84268.150137	37.127322
1694.963943	84349.667261	37.132340
1696.790948	84445.897422	37.137357
1698.532445	84534.297818	37.142375
1700.458186	84607.261437	37.147392
1701.573284	84695.481594	37.152410
1703.476840	84789.597498	37.157428
1705.385808	84875.945328	37.162445
1706.713702	84970.544727	37.167463
1708.720328	85052.164048	37.172480
1710.653839	85148.582638	37.177498
1712.137325	85242.005475	37.182516
1714.308987	85329.466662	37.187533
1715.843986	85425.099550	37.192551
1717.502350	85488.274100	37.197568
1719.072303	85591.644426	37.202586
1720.862041	85688.708233	37.207604
1722.816816	85774.303955	37.212621
1724.508581	85863.476517	37.217639
1726.861613	85936.794805	37.222656
1728.604788	86030.990546	37.227674
1730.160662	86124.759717	37.232692
1731.601359	86203.607013	37.237709
1733.186064	86288.476511	37.242727
1735.168398	86384.726846	37.247744
1736.754711	86469.026379	37.252762
1738.577429	86554.771793	37.257780
1740.256118	86637.169218	37.262797
1741.966178	86726.265534	37.267815
1743.839746	86814.740941	37.272832
1745.549562	86897.919907	37.277850
1747.171228	86991.871659	37.282868
1749.632595	87074.109817	37.287885
1750.611738	87164.475035	37.292903
1752.727890	87252.128120	37.297920
1754.156648	87338.368351	37.302938
1756.116955	87421.750385	37.307956
1758.336759	87506.587400	37.312973
1760.110231	87588.605174	37.317991
1761.490705	87662.434845	37.323008
1763.298027	87754.851957	37.328026
1765.549337	87835.477694	37.333044
1767.254210	87906.063708	37.338061
1768.651302	87973.491868	37.343079
1770.444782	88034.217646	37.348096
1771.877735	88094.214261	37.353114
1773.551523	88158.520068	37.358132
1775.283794	88224.464328	37.363149
1776.569185	88300.667622	37.368167
1778.321639	88371.576803	37.373184
1779.761957	88473.013319	37.378202
1781.369442	88550.611565	37.383220
1782.865023	88642.041067	37.388237
1784.474226	88736.519940	37.393255
1786.388793	88822.713843	37.398272
1788.208360	88921.279129	37.403290
1789.931104	89014.727274	37.408308
1792.072465	89122.228124	37.413325
1793.773541	89218.975331	37.418343
1795.522052	89314.891668	37.423360
1797.316573	89411.536166	37.428378
1799.230649	89515.778949	37.433396
1801.063720	89607.412079	37.438413
1802.706762	89718.604984	37.443431
1804.498661	89818.901163	37.448448
1806.330390	89924.526999	37.453466
1808.261644	90023.914913	37.458484
1810.677211	90120.768690	37.463501
1812.103498	90233.923820	37.468519
1814.280874	90336.290587	37.473536
1816.376904	90431.902659	37.478554
1818.068290	90523.003126	37.483572
1820.166433	90616.625675	37.488589
1822.034880	90706.469632	37.493607
1823.983032	90806.009585	37.498624
1826.175479	90901.354589	37.503642
1827.999736	90989.546023	37.508660
1830.078740	91075.505249	37.513677
1831.854213	91160.840495	37.518695
1834.247475	91246.801729	37.523712
1835.836113	91350.899043	37.528730
1837.443627	91425.032051	37.533748
1839.634149	91511.583431	37.538765
1841.111417	91607.308745	37.543783
1842.981452	91689.626898	37.548800
1844.580092	91777.310950	37.553818
1846.360929	91880.644902	37.558836
1848.632048	91971.405544	37.563853
1850.104043	92070.479184	37.568871
1852.081053	92166.343527	37.573888
1853.738022	92263.905941	37.578906
1855.531012	92364.235781	37.583924
1857.606623	92453.672284	37.588941
1858.944119	92557.876416	37.593959
1861.216778	92651.883555	37.598976
1862.983946	92755.678910	37.603994
1864.564107	92857.780116	37.609012
1866.913257	92955.097006	37.614029
1868.498240	93057.540344	37.619047
1870.612843	93155.110047	37.624064
1872.483952	93249.638161	37.629082
1874.314992	93357.037912	37.634100
1875.921733	93446.715472	37.639117
1877.585729	93549.604391	37.644135
1879.260767	93651.579322	37.649152
1881.394211	93765.625623	37.654170
1882.919210	93870.058381	37.659188
1884.869074	93974.703863	37.664205
1886.537877	94086.250994	37.669223
1888.672949	94192.021681	37.674240
1890.378001	94289.380220	37.679258
1892.149289	94388.477903	37.684276
1894.235255	94469.616302	37.689293
1896.118725	94568.773062	37.694311
1897.602282	94653.200424	37.699328
1899.571672	94732.887401	37.704346
1900.989253	94849.648210	37.709364
1902.854602	94940.303692	37.714381
1904.629396	95051.596882	37.719399
1906.370777	95153.376255	37.724416
1908.161122	95262.538251	37.729434
1910.150146	95380.403154	37.734452
1912.051530	95480.713522	37.739469
1913.689357	95601.600358	37.744487
1916.006886	95717.146149	37.749504
1917.840223	95824.211859	37.754522
1919.809281	95949.839726	37.759540
1921.632961	96054.714787	37.764557
1923.452384	96178.490930	37.769575
1925.552072	96301.019472	37.774592
1927.802629	96422.193884	37.779610
1929.682238	96549.562116	37.784628
1932.046917	96664.825149	37.789645
1933.617290	96792.787835	37.794663
1935.508161	96918.457166	37.799680
1937.637088	97031.096386	37.804698
1939.433039	97160.685881	37.809716
1941.287197	97275.308472	37.814733
1942.933507	97403.020893	37.819751
1944.932131	97530.437844	37.824768
1947.109583	97667.930654	37.829786
1949.275165	97795.981736	37.834804
1951.369674	97932.867511	37.839821
1953.137966	98060.195862	37.844839
1955.519967	98179.353503	37.849856
1957.234334	98302.393790	37.854874
1959.291130	98441.506121	37.859892
1961.162436	98561.049348	37.864909
1962.944301	98704.135730	37.869927
1965.010322	98843.045531	37.874944
1967.588587	98961.858454	37.879962
1969.376950	99101.129751	37.884980
1971.359511	99226.248730	37.889997
1973.493956	99359.698816	37.895015
1975.003295	99501.196015	37.900032
1977.045610	99621.299597	37.905050
1979.024461	99762.192021	37.910068
1981.050800	99889.297099	37.915085
1983.121001	100027.564806	37.920103
1985.217039	100152.618915	37.925120
1987.617612	100276.839837	37.930138
1989.414505	100418.410156	37.935156
1991.472254	100546.362312	37.940173
1993.529826	100673.414870	37.945191
1995.418087	100811.067816	37.950208
1997.713302	100938.616700	37.955226
1999.439255	101068.144185	37.960244
2001.533293	101193.659026	37.965261
2003.203496	101327.696985	37.970279
2005.374962	101448.661918	37.975296
2007.467087	101582.875790	37.980314
2009.389845	101727.348094	37.985332
2011.370646	101855.925985	37.990349
2013.354691	101982.373903	37.995367
2015.049260	102116.664844	38.000384
2017.120078	102243.620006	38.005402
2018.972216	102387.053945	38.010420
2020.808219	102520.918689	38.015437
2022.940044	102655.929483	38.020455
2024.884465	102786.304390	38.025472
2026.888410	102903.446565	38.030490
2028.582773	103034.495513	38.035508
2030.063626	103156.969453	38.040525
2032.202816	103277.020600	38.045543
2033.830895	103415.523932	38.050560
2036.048247	103554.620302	38.055578
2037.319613	103695.513547	38.060596
2039.316554	103833.390343	38.065613
2041.496187	103989.763367	38.070631
2043.314118	104135.581215	38.075648
2045.191308	104292.446749	38.080666
2047.315891	104456.285978	38.085684
2049.276597	104609.843302	38.090701
2051.650266	104779.059233	38.095719
2053.715131	104928.189264	38.100736
2055.998382	105085.337312	38.105754
2057.480332	105259.145707	38.110772
2059.784070	105416.862675	38.115789
2062.085919	105578.409961	38.120807
2063.912675	105747.120369	38.125824
2066.524049	105907.644448	38.130842
2068.903024	106069.258084	38.135860
2070.877637	106233.433716	38.140877
2073.199667	106390.721230	38.145895
2075.082987	106553.175519	38.150912
2077.256403	106707.228954	38.155930
2079.564016	106882.704364	38.160948
2081.664239	107051.530602	38.165965
2084.022041	107213.102244	38.170983
2085.642129	107381.409251	38.176000
2088.294017	107541.807867	38.181018
2089.840006	107711.548295	38.186036
2091.856440	107880.176140	38.191053
2094.155578	108041.418470	38.196071
2096.439040	108223.270186	38.201088
2098.579641	108376.917767	38.206106
2100.946314	108554.408690	38.211124
2102.723912	108711.601783	38.216141
2105.330248	108887.116728	38.221159
2107.234249	109063.680843	38.226176
2109.316305	109225.812266	38.231194
2111.537944	109392.589266	38.236212
2113.709533	109567.947394	38.241229
2116.069707	109734.615580	38.246247
2117.761148	109904.584884	38.251264
2120.298565	110065.000368	38.256282
2122.008675	110236.147723	38.261300
2123.893549	110411.986089	38.266317
2126.079075	110583.935770	38.271335
2127.816170	110769.031227	38.276352
2130.470288	110929.559198	38.281370
2132.536614	111118.460206	38.286388
2134.223845	111302.754613	38.291405
2136.538886	111481.130752	38.296423
2138.146454	111660.239891	38.301440
2140.697048	111844.072283	38.306458
2142.960502	112043.701712	38.311476
2144.865345	112230.985198	38.316493
2146.813261	112403.868589	38.321511
2148.711775	112598.269710	38.326528
2150.639700	112780.974139	38.331546
2152.554733	112976.541491	38.336564
2155.077740	113167.106652	38.341581
2157.435087	113360.729868	38.346599
2159.398033	113561.264447	38.351616
2162.221771	113749.756398	38.356634
2163.993655	113937.640247	38.361652
2165.969872	114107.014216	38.366669
2168.372899	114267.000277	38.371687
2170.174839	114438.089870	38.376704
2172.283799	114596.576062	38.381722
2174.485119	114768.695451	38.386740
2176.336626	114946.615827	38.391757
2178.596778	115123.001880	38.396775
2180.804015	115302.872263	38.401792
2182.801777	115487.824248	38.406810
2184.716037	115673.475124	38.411828
2186.507321	115855.810429	38.416845
2189.025117	116041.685809	38.421863
2191.002508	116241.192703	38.426880
2193.419011	116435.761453	38.431898
2195.782561	116634.322181	38.436916
2197.818410	116836.309114	38.441933
2200.154939	117026.365351	38.446951
2202.111602	117231.258711	38.451968
2204.508439	117427.839749	38.456986
2206.881644	117635.447929	38.462004
2209.036991	117839.362211	38.467021
2211.252739	118045.246873	38.472039
2213.287860	118255.930185	38.477056
2215.699380	118447.186850	38.482074
2218.345112	118664.448839	38.487092
2220.192912	118856.239707	38.492109
2222.691672	119061.603587	38.497127
2225.107485	119274.325914	38.502144
2227.559950	119487.272012	38.507162
2229.673171	119695.515598	38.512180
2232.085316	119905.375251	38.517197
2234.388439	120114.656915	38.522215
2236.234337	120331.736361	38.527232
2238.117673	120527.563812	38.532250
2240.242069	120750.855732	38.537268
2242.573344	120978.366086	38.542285
2244.973034	121194.006401	38.547303
2247.216439	121405.042234	38.552320
2249.633801	121628.673904	38.557338
2251.868665	121846.956786	38.562356
2254.391161	122066.603970	38.567373
2256.682577	122285.134146	38.572391
2259.030365	122508.109367	38.577408
2261.298734	122732.645926	38.582426
2263.148022	122954.699481	38.587444
2265.326014	123176.817025	38.592461
2267.817141	123399.470371	38.597479
2269.912859	123626.741087	38.602496
2272.308857	123856.059316	38.607514
2274.344482	124087.338154	38.612532
2277.011449	124314.726380	38.617549
2279.784402	124533.815178	38.622567
2281.848723	124757.570423	38.627584
2284.432127	124974.623394	38.632602
2286.720232	125190.543884	38.637620
2289.042437	125415.695989	38.642637
2291.474311	125641.606067	38.647655
2293.408508	125872.099026	38.652672
2295.589085	126084.108202	38.657690
2297.745403	126311.397197	38.662708
2299.770616	126550.202283	38.667725
2302.286842	126760.284779	38.672743
2304.323310	126992.239708	38.677760
2306.538256	127223.952336	38.682778
2308.755362	127437.561333	38.687796
2310.919868	127688.543564	38.692813
2313.328727	127922.551515	38.697831
2315.588412	128149.732928	38.702848
2317.663378	128369.395440	38.707866
2319.742256	128577.385980	38.712884
2322.113516	128805.961805	38.717901
2324.340580	129012.979746	38.722919
2326.090315	129229.982473	38.727936
2327.799416	129462.129181	38.732954
2330.463153	129690.955853	38.737972
2332.586253	129931.414335	38.742989
2334.658886	130163.457246	38.748007
2336.623748	130413.053166	38.753024
2339.246597	130652.117961	38.758042
2341.714900	130908.908304	38.763060
2343.851552	131155.373049	38.768077
2346.543281	131409.949038	38.773095
2348.752564	131660.008786	38.778112
2351.294854	131917.821304	38.783130
2353.597691	132166.828873	38.788148
2355.949039	132436.055973	38.793165
2358.827713	132682.920836	38.798183
2361.166168	132946.062498	38.803200
2363.570791	133201.036437	38.808218
2365.898041	133450.377373	38.813236
2368.465963	133716.190469	38.818253
2371.171635	133979.889906	38.823271
2373.103596	134234.626499	38.828288
2375.621596	134503.167580	38.833306
2378.053015	134758.539619	38.838324
2380.226908	135037.720616	38.843341
2382.369679	135297.023816	38.848359
2384.902437	135574.350087	38.853376
2387.472649	135851.228058	38.858394
2389.934289	136113.493483	38.863412
2392.056067	136394.239120	38.868429
2394.709565	136663.901205	38.873447
2397.102457	136948.364016	38.878464
2399.817309	137215.266024	38.883482
2402.296644	137500.848128	38.888500
2404.649027	137776.553535	38.893517
2406.997408	138055.560660	38.898535
2409.462756	138331.238987	38.903552
2411.943599	138611.459668	38.908570
2413.866313	138902.822714	38.913588
2416.446290	139194.681196	38.918605
2419.270267	139454.104198	38.923623
2421.818777	139734.206745	38.928640
2424.358696	140016.418949	38.933658
2427.009189	140289.516204	38.938676
2429.168754	140572.514566	38.943693
2431.495860	140846.223978	38.948711
2433.714540	141133.087133	38.953728
2435.955959	141420.379929	38.958746
2438.609829	141705.211270	38.963764
2440.401850	141989.849122	38.968781
2442.884364	142286.564306	38.973799
2445.631976	142593.925992	38.978816
2448.291976	142868.495780	38.983834
2450.763066	143165.332271	38.988852
2453.362958	143446.907726	38.993869
2455.961337	143737.635738	38.998887
2458.675212	144022.851831	39.003904
2461.012612	144306.973481	39.008922
2463.644417	144583.841666	39.013940
2465.748475	144874.843969	39.018957
2468.408748	145161.102945	39.023975
2470.719677	145449.512385	39.028992
2472.715834	145734.507719	39.034010
2475.495511	146020.993995	39.039028
2477.402616	146326.263439	39.044045
2479.646571	146590.904292	39.049063
2481.907087	146870.939902	39.054080
2483.843588	147145.239897	39.059098
2486.253500	147425.585128	39.064116
2488.526613	147717.795549	39.069133
2490.717612	148009.855435	39.074151
2493.173150	148309.465877	39.079168
2495.166110	148611.282784	39.084186
2497.324619	148918.711195	39.089204
2499.635954	149241.196829	39.094221
2502.029810	149552.755396	39.099239
2504.327840	149888.117840	39.104256
2506.564725	150211.674473	39.109274
2509.304730	150548.190424	39.114292
2511.678590	150881.376575	39.119309
2514.114759	151220.698673	39.124327
2516.750315	151566.389251	39.129344
2518.887406	151926.237261	39.134362
2521.422195	152274.080555	39.139380
2524.293028	152625.922789	39.144397
2526.600164	152976.078255	39.149415
2529.127626	153342.678253	39.154432
2531.564599	153713.737708	39.159450
2534.116557	154063.506163	39.164468
2536.804279	154439.596086	39.169485
2539.819703	154795.745189	39.174503
2542.330240	155159.325524	39.179520
2544.749755	155532.316292	39.184538
2547.305433	155896.211524	39.189556
2549.923469	156275.700979	39.194573
2552.493203	156641.058497	39.199591
2555.485625	157023.363190	39.204608
2557.666297	157403.423360	39.209626
2560.433192	157776.373917	39.214644
2562.671764	158165.417875	39.219661
2565.275531	158558.291911	39.224679
2567.983763	158930.179641	39.229696
2569.994511	159317.057598	39.234714
2573.081932	159713.379959	39.239732
2575.747644	160103.867425	39.244749
2578.423218	160492.019808	39.249767
2580.755709	160878.082691	39.254784
2583.157211	161278.572126	39.259802
2585.873639	161685.667398	39.264820
2588.370576	162081.576459	39.269837
2590.713771	162485.446948	39.274855
2593.643380	162888.085583	39.279872
2595.806611	163293.538141	39.284890
2598.794874	163701.987403	39.289908
2601.493842	164106.358157	39.294925
2603.876399	164525.356224	39.299943
2606.399349	164923.411291	39.304960
2608.813878	165352.198415	39.309978
2611.491552	165764.809766	39.314996
2613.850427	166186.399193	39.320013
2616.623949	166617.893248	39.325031
2619.081876	167028.565837	39.330048
2620.979802	167461.217802	39.335066
2623.855884	167883.523784	39.340084
2626.439635	168324.199783	39.345101
2628.795827	168752.407455	39.350119
2631.244843	169189.021365	39.355136
2634.057506	169635.421376	39.360154
2636.597753	170073.321420	39.365172
2638.841678	170515.866861	39.370189
2641.693187	170961.887884	39.375207
2644.285423	171399.952658	39.380224
2646.907133	171843.234074	39.385242
2649.952474	172254.352056	39.390260
2652.436800	172679.806860	39.395277
2655.090120	173095.612616	39.400295
2657.754336	173512.218846	39.405312
2659.693155	173953.981104	39.410330
2662.598460	174372.738201	39.415348
2665.181691	174801.680937	39.420365
2667.535785	175235.944221	39.425383
2670.002626	175669.125532	39.430400
2672.746594	176120.691002	39.435418
2675.206239	176561.471694	39.440436
2677.737163	177013.088015	39.445453
2680.260447	177470.523853	39.450471
2682.860241	177925.740625	39.455488
2685.593031	178389.650261	39.460506
2687.887936	178866.583533	39.465524
2690.314457	179344.565501	39.470541
2692.508504	179839.679038	39.475559
2695.302499	180310.548140	39.480576
2698.030336	180815.056918	39.485594
2700.852843	181304.441796	39.490612
2703.169903	181813.693526	39.495629
2706.205842	182315.622443	39.500647
2709.054005	182819.793048	39.505664
2711.690887	183326.412212	39.510682
2714.417032	183859.053785	39.515700
2716.765692	184419.823067	39.520717
2719.709184	184952.004726	39.525735
2722.794276	185457.548699	39.530752
2725.716409	185978.055439	39.535770
2729.359063	186476.887983	39.540788
2732.534386	186985.117616	39.545805
2735.209067	187487.001859	39.550823
2737.996115	187999.056169	39.555840
2740.870584	188515.721980	39.560858
2743.672898	189015.612069	39.565876
2746.662097	189515.297346	39.570893
2749.306494	190031.371089	39.575911
2752.232151	190532.670937	39.580928
2754.773850	191062.786292	39.585946
2757.571354	191557.989011	39.590964
2760.077861	192081.510212	39.595981
2762.677746	192602.936171	39.600999
2765.873465	193114.847386	39.606016
2768.042210	193639.012154	39.611034
2770.667086	194167.883112	39.616052
2773.460169	194695.815450	39.621069
2775.875504	195220.989409	39.626087
2778.829796	195758.603988	39.631104
2781.088049	196305.143830	39.636122
2783.486974	196850.342905	39.641140
2786.231180	197388.885608	39.646157
2789.014980	197941.064850	39.651175
2792.496652	198491.308049	39.656192
2795.346816	199034.895080	39.661210
2798.196996	199577.671139	39.666228
2801.061351	200123.393481	39.671245
2803.589573	200676.638476	39.676263
2806.481731	201232.800462	39.681280
2809.114193	201798.759398	39.686298
2811.667616	202345.172637	39.691316
2814.454747	202914.006845	39.696333
2817.289989	203478.593059	39.701351
2819.898771	204034.147629	39.706368
2822.965686	204606.270962	39.711386
2825.306460	205177.874445	39.716404
2828.162929	205741.092128	39.721421
2830.699701	206302.278281	39.726439
2833.632547	206837.746882	39.731456
2836.482324	207387.734936	39.736474
2839.264240	207925.287377	39.741492
2842.515146	208476.866482	39.746509
2844.931491	209008.813611	39.751527
2847.798459	209549.049083	39.756544
2850.023836	210105.872809	39.761562
2852.534624	210669.359553	39.766580
2855.692239	211225.049015	39.771597
2857.925631	211813.730842	39.776615
2860.274097	212389.948057	39.781632
2862.647123	212989.940266	39.786650
2865.278417	213574.625560	39.791668
2868.135667	214173.959835	39.796685
2871.115351	214788.645205	39.801703
2874.203445	215392.111516	39.806720
2877.023254	216004.181752	39.811738
2879.871644	216621.608579	39.816756
2882.880162	217235.378411	39.821773
2885.914862	217862.786792	39.826791
2889.014855	218475.044921	39.831808
2891.977567	219105.285748	39.836826
2895.154628	219728.380530	39.841844
2898.483048	220346.320555	39.846861
2901.465982	220966.779259	39.851879
2904.325073	221595.666473	39.856896
2907.061731	222232.753294	39.861914
2909.797794	222863.311661	39.866932
2913.189776	223496.028644	39.871949
2915.883835	224143.132040	39.876967
2918.800940	224772.671846	39.881984
2921.558098	225426.446807	39.887002
2923.857929	226073.002295	39.892020
2927.086833	226728.837318	39.897037
2930.085534	227384.631972	39.902055
2932.998534	228038.458285	39.907072
2936.212860	228702.957692	39.912090
2939.042063	229364.112811	39.917108
2942.444253	230016.540516	39.922125
2945.393863	230670.410315	39.927143
2948.746951	231326.731441	39.932160
2951.739946	231978.179872	39.937178
2954.610842	232637.979183	39.942196
2957.573119	233298.144472	39.947213
2959.940556	233971.789754	39.952231
2963.131930	234636.312266	39.957248
2965.822971	235303.985862	39.962266
2968.349768	235986.189574	39.967284
2971.645625	236663.267268	39.972301
2974.650694	237354.665995	39.977319
2977.119182	238029.685696	39.982336
2980.427384	238717.096592	39.987354
2983.038481	239415.919483	39.992372
2985.920422	240111.903951	39.997389
2988.689319	240818.040263	40.002407
2991.384403	241517.454350	40.007424
2994.508331	242225.157076	40.012442
2997.329484	242932.905066	40.017460
3000.663620	243639.478335	40.022477
3003.492709	244347.169854	40.027495
3006.791185	245050.670364	40.032512
3010.366402	245755.268321	40.037530
3013.420300	246467.464503	40.042548
3016.475256	247167.236014	40.047565
3019.076675	247884.755956	40.052583
3022.601994	248582.035274	40.057600
3025.817623	249281.849665	40.062618
3029.389217	249976.220244	40.067636
3032.501059	250634.792060	40.072653
3035.191512	251297.948625	40.077671
3038.422534	251944.862264	40.082688
3041.773159	252609.561095	40.087706
3043.995795	253260.945082	40.092724
3047.489852	253921.043276	40.097741
3049.949151	254576.575556	40.102759
3052.920145	255232.888377	40.107776
3055.902712	255913.886157	40.112794
3058.811896	256573.377252	40.117812
3061.986609	257254.769869	40.122829
3064.411958	257955.174193	40.127847
3067.087663	258634.910137	40.132864
3070.225732	259333.467954	40.137882
3073.134854	260043.894048	40.142900
3075.656081	260753.360490	40.147917
3078.302923	261472.937515	40.152935
3081.276387	262204.244396	40.157952
3084.265409	262938.388767	40.162970
3086.962567	263685.197349	40.167988
3089.988143	264435.835420	40.173005
3093.109858	265192.218650	40.178023
3096.369753	265967.496879	40.183040
3099.687074	266719.190106	40.188058
3102.836866	267485.736536	40.193076
3106.183825	268234.822795	40.198093
3109.283145	269017.467404	40.203111
3112.194113	269792.337737	40.208128
3115.651325	270563.484232	40.213146
3118.080226	271352.055206	40.218164
3121.549320	272137.002478	40.223181
3124.901489	272918.913311	40.228199
3128.292494	273697.077603	40.233216
3132.018877	274482.699643	40.238234
3135.005435	275267.769617	40.243252
3138.723397	276048.806676	40.248269
3142.315842	276818.808588	40.253287
3145.874055	277600.109385	40.258304
3149.589320	278360.934568	40.263322
3152.847031	279124.414058	40.268340
3156.332544	279892.624454	40.273357
3159.879379	280639.054236	40.278375
3163.091829	281409.196211	40.283392
3166.264521	282166.055172	40.288410
3169.258362	282933.370936	40.293428
3172.283330	283677.616242	40.298445
3175.225554	284448.504015	40.303463
3177.816566	285220.225262	40.308480
3181.176648	285987.551544	40.313498
3183.829703	286763.028978	40.318516
3187.213154	287547.244955	40.323533
3189.857049	288330.805427	40.328551
3192.795679	289115.554501	40.333568
3195.640666	289919.199545	40.338586
3198.604210	290712.507165	40.343604
3202.069728	291516.415570	40.348621
3205.320837	292329.766726	40.353639
3208.246440	293142.827833	40.358656
3211.252124	293946.090494	40.363674
3213.788304	294769.498449	40.368692
3217.246334	295599.402548	40.373709
3220.335656	296425.924993	40.378727
3223.271923	297249.438282	40.383744
3226.168008	298094.347620	40.388762
3229.164692	298931.866191	40.393780
3232.662901	299777.569774	40.398797
3235.677177	300635.724524	40.403815
3238.499188	301467.621200	40.408832
3242.261292	302286.284354	40.413850
3245.338242	303112.378306	40.418868
3248.428581	303927.440117	40.423885
3251.556193	304747.991704	40.428903
3254.509794	305564.825919	40.433920
3257.733164	306385.209285	40.438938
3260.667360	307228.900858	40.443956
3264.056364	308064.029166	40.448973
3267.614635	308900.462103	40.453991
3270.851502	309733.428236	40.459008
3274.618460	310572.414035	40.464026
3277.639602	311420.029725	40.469044
3281.205462	312261.809056	40.474061
3284.217742	313114.344827	40.479079
3287.720093	313980.873985	40.484096
3290.568201	314837.870403	40.489114
3293.669836	315706.662862	40.494132
3297.054257	316563.517382	40.499149
3300.281854	317453.472427	40.504167
3303.496238	318335.214806	40.509184
3307.317928	319218.189431	40.514202
3310.306675	320110.005685	40.519220
3313.480572	320994.009552	40.524237
3316.668547	321889.081747	40.529255
3319.668064	322783.149425	40.534272
3323.448706	323688.950845	40.539290
3326.934891	324599.802405	40.544308
3330.276518	325504.414620	40.549325
3333.468391	326423.593778	40.554343
3336.670925	327334.605981	40.559360
3340.452835	328249.895995	40.564378
3343.852346	329177.453184	40.569396
3346.910574	330103.671804	40.574413
3350.458449	331036.362424	40.579431
3353.610151	331956.661743	40.584448
3356.938613	332886.018361	40.589466
3360.485917	333821.127071	40.594484
3363.881858	334764.429596	40.599501
3368.133530	335685.379027	40.604519
3371.935190	336608.582601	40.609536
3376.249900	337523.794171	40.614554
3379.513229	338435.621384	40.619572
3382.830875	339352.819429	40.624589
3386.492058	340275.063488	40.629607
3389.743844	341191.235211	40.634624
3393.150197	342111.365988	40.639642
3396.967877	343014.898179	40.644660
3400.817440	343906.989634	40.649677
3404.627174	344813.696597	40.654695
3407.924797	345717.112085	40.659712
3411.633860	346615.925311	40.664730
3415.301046	347515.177417	40.669748
3418.256351	348408.912643	40.674765
3421.933069	349307.632849	40.679783
3424.861847	350206.825685	40.684800
3428.499530	351093.459000	40.689818
3431.958665	351990.389667	40.694836
3435.526681	352894.909604	40.699853
3438.891073	353792.032716	40.704871
3441.890649	354695.423997	40.709888
3445.020485	355593.191667	40.714906
3448.395447	356507.803939	40.719924
3451.743865	357420.847020	40.724941
3455.480056	358324.626045	40.729959
3459.069482	359228.147790	40.734976
3462.920440	360140.118479	40.739994
3466.070566	361039.801944	40.745012
3469.754953	361921.260015	40.750016
3472.918332	362780.831269	40.755021
3475.621996	363605.155862	40.760026
3479.139391	364358.567054	40.765031
3482.124611	365089.098564	40.770036
3484.543253	365748.661134	40.775040
3487.377401	366364.697918	40.780045
3489.435380	366937.372538	40.785050
3492.398786	367442.416032	40.790055
3494.440998	367927.270198	40.795060
3496.691900	368341.863725	40.800064
3498.758852	368711.056168	40.805069
3500.358438	369044.420294	40.810074
3502.700810	369311.968966	40.815079
3504.251700	369571.865195	40.820084
3506.107243	369768.405024	40.825088
3507.650453	369943.424563	40.830093
3508.726168	370070.604956	40.835098
3510.306331	370159.549855	40.840103
3511.599234	370247.447033	40.845108
3513.018791	370277.404424	40.850112
3513.937293	370276.905236	40.855117
3514.821361	370263.303270	40.860122
3515.549366	370216.472584	40.865127
3516.440970	370150.309574	40.870132
3517.552548	370070.673520	40.875136
3518.273337	369954.567841	40.880141
3518.717882	369824.939235	40.885146
3519.544639	369686.155670	40.890151
3519.659202	369536.228759	40.895156
3519.815917	369360.432962	40.900160
3520.612500	369177.346592	40.905165
3520.683511	368991.552562	40.910170
3520.972229	368774.145176	40.915175
3521.274780	368565.701907	40.920180
3521.588649	368347.703006	40.925184
3521.986435	368114.496918	40.930189
3522.082290	367879.888006	40.935194
3522.649966	367630.468050	40.940199
3522.648355	367385.835028	40.945204
3522.592862	367117.275671	40.950208
3523.123832	366860.156650	40.955213
3522.933864	366585.820666	40.960218
3523.305848	366301.307652	40.965223
3523.193671	366020.526161	40.970228
3523.185144	365741.758332	40.975232
3523.406616	365458.251437	40.980237
3522.857443	365167.112826	40.985242
3522.883365	364883.986607	40.990247
3522.881624	364598.626016	40.995252
3522.745493	364314.299994	41.000256
3523.221889	364023.294529	41.005261
3522.742521	363719.883448	41.010266
3522.914343	363429.275438	41.015271
3522.749673	363140.978629	41.020276
3522.617676	362842.281218	41.025280
3522.530950	362544.615530	41.030285
3522.604455	362257.899127	41.035290
3522.603106	361963.034817	41.040295
3522.670304	361660.152410	41.045300
3522.637344	361363.101759	41.050304
3522.450938	361065.081096	41.055309
3522.403644	360768.789129	41.060314
3522.241172	360472.613892	41.065319
3522.179088	360175.378142	41.070324
3522.128463	359881.390470	41.075328
3521.816775	359582.764807	41.080333
3521.378373	359280.293234	41.085338
3521.340817	358995.926444	41.090343
3521.127679	358721.724417	41.095348
3520.957664	358436.280330	41.100352
3520.730198	358141.896850	41.105357
3520.471598	357865.305332	41.110362
3521.021842	357587.060004	41.115367
3520.631894	357302.808805	41.120372
3519.948225	357026.047457	41.125376
3520.158258	356740.121550	41.130381
3519.709910	356470.637986	41.135386
3519.711906	356198.743444	41.140391
3519.642898	355940.658381	41.145396
3519.073874	355670.958004	41.150400
3519.065504	355405.844223	41.155405
3518.814576	355145.315650	41.160410
3519.308143	354880.118945	41.165415
3518.966491	354617.897261	41.170420
3518.715915	354366.258056	41.175424
3518.799375	354098.882182	41.180429
3518.662425	353849.356138	41.185434
3518.477399	353593.074548	41.190439
3517.990006	353343.268875	41.195444
3518.057809	353089.765076	41.200448
3517.979938	352842.433250	41.205453
3517.717226	352601.991385	41.210458
3517.485838	352359.077205	41.215463
3517.599770	352111.862251	41.220468
3517.378724	351869.196930	41.225472
3517.399835	351627.101980	41.230477
3516.861984	351399.734172	41.235482
3517.061919	351155.802948	41.240487
3516.746606	350921.152396	41.245492
3516.693323	350694.415623	41.250496
3516.577147	350448.698258	41.255501
3516.548084	350231.080294	41.260506
3516.181323	349997.295400	41.265511
3515.856471	349770.391281	41.270516
3515.641172	349553.738479	41.275520
3515.737855	349335.789841	41.280525
3515.648968	349121.834469	41.285530
3515.415077	348897.020039	41.290535
3515.326958	348693.738727	41.295540
3515.154396	348476.207809	41.300544
3515.611763	348254.611170	41.305549
3514.925364	348047.911202	41.310554
3514.824168	347842.008232	41.315559
3514.816188	347638.911289	41.320564
3514.345156	347439.266686	41.325568
3514.557506	347241.141096	41.330573
3514.582626	347042.484301	41.335578
3513.897307	346828.403985	41.340583
3514.167125	346640.918061	41.345588
3514.037167	346443.705650	41.350592
3514.041253	346253.106624	41.355597
3513.613683	346062.472308	41.360602
3513.758578	345871.060978	41.365607
3513.453245	345687.981683	41.370612
3513.171447	345498.821397	41.375616
3513.198758	345307.120170	41.380621
3512.926159	345130.083670	41.385626
3513.020158	344951.514323	41.390631
3512.552792	344776.820049	41.395636
3512.379345	344595.951596	41.400640
3512.354137	344429.932482	41.405645
3512.229498	344256.097249	41.410650
3512.463312	344081.315219	41.415655
3512.492170	343913.556248	41.420660
3512.227360	343741.876030	41.425664
3512.044194	343575.216414	41.430669
3511.806941	343425.167287	41.435674
3511.700844	343243.899791	41.440679
3511.994074	343085.452076	41.445684
3511.709999	342927.017612	41.450688
3512.021156	342767.599457	41.455693
3511.752550	342600.897643	41.460698
3511.487031	342435.872676	41.465703
3511.426116	342291.562813	41.470708
3511.220187	342132.934521	41.475712
3511.239877	341979.152130	41.480717
3511.005243	341825.612235	41.485722
3511.303258	341669.801690	41.490727
3510.811356	341514.546202	41.495732
3510.577805	341373.666736	41.500736
3510.774394	341222.752039	41.505741
3510.446241	341080.970812	41.510746
3510.410164	340943.669409	41.515751
3510.090957	340811.904049	41.520756
3510.298453	340667.952371	41.525760
3510.643022	340526.292587	41.530765
3509.909657	340386.555268	41.535770
3509.956020	340257.909149	41.540775
3509.679462	340108.869030	41.545780
3509.469475	339976.676635	41.550784
3509.723816	339840.190094	41.555789
3509.561099	339718.974280	41.560794
3509.441712	339593.072480	41.565799
3509.475794	339459.339737	41.570804
3509.094260	339332.766006	41.575808
3509.428730	339210.428167	41.580813
3508.955343	339095.768508	41.585818
3509.022480	338971.793358	41.590823
3509.067686	338850.694662	41.595828
3508.624054	338729.722838	41.600832
3508.734567	338608.816546	41.605837
3509.001575	338494.954655	41.610842
3508.987065	338366.845248	41.615847
3508.494016	338260.119879	41.620852
3508.286857	338145.822430	41.625856
3508.461879	338033.677225	41.630861
3508.495683	337917.942768	41.635866
3508.349324	337799.769443	41.640871
3508.387711	337694.052787	41.645876
3508.030982	337590.253960	41.650880
3508.090099	337467.495515	41.655885
3507.838796	337373.470043	41.660890
3507.750433	337261.389055	41.665895
3507.946993	337161.978167	41.670900
3507.776535	337064.099329	41.675904
3508.046902	336955.724963	41.680909
3507.866512	336859.398366	41.685914
3507.815735	336754.989859	41.690919
3507.811736	336645.970850	41.695924
3507.748388	336544.030449	41.700928
3507.558500	336439.668220	41.705933
3507.363373	336345.783900	41.710938
3507.385719	336252.094215	41.715943
3507.653515	336154.093564	41.720948
3507.011712	336060.608945	41.725952
3507.515072	335958.883488	41.730957
3507.383883	335872.286604	41.735962
3507.060733	335779.819550	41.740967
3507.014892	335677.746852	41.745972
3506.952487	335594.851489	41.750976
3507.334731	335502.527770	41.755981
3506.764737	335411.929426	41.760986
3506.939049	335322.130021	41.765991
3506.881310	335232.519265	41.770996
3506.815426	335148.733350	41.776000
3506.662611	335060.917238	41.781005
3506.420958	334978.989482	41.786010
3506.036902	334897.592438	41.791015
3506.295206	334820.316436	41.796020
3506.227272	334739.759730	41.801024
3506.370740	334655.838246	41.806029
3506.311585	334583.011068	41.811034
3506.275401	334498.252636	41.816039
3506.401177	334415.706696	41.821044
3506.176539	334341.607891	41.826048
3505.942811	334249.936863	41.831053
3506.166328	334180.320000	41.836058
3505.942656	334106.907244	41.841063
3505.820122	334037.013598	41.846068
3505.489379	333970.204234	41.851072
3505.625144	333884.247648	41.856077
3505.728380	333836.317206	41.861082
3505.698761	333760.228477	41.866087
3505.605716	333691.524896	41.871092
3505.512668	333621.956487	41.876096
3505.808156	333542.688305	41.881101
3505.630376	333485.620228	41.886106
3505.586372	333410.397745	41.891111
3505.744354	333337.559631	41.896116
3505.522508	333277.064727	41.901120
3505.540469	333213.073389	41.906125
3505.393464	333142.418925	41.911130
3505.646150	333083.350054	41.916135
3505.336709	333007.074655	41.921140
3505.147011	332954.661846	41.926144
3505.322201	332877.928928	41.931149
3504.964788	332833.070311	41.936154
3504.814040	332756.820464	41.941159
3505.055957	332698.363067	41.946164
3505.083487	332637.904452	41.951168
3505.041928	332585.696870	41.956173
3505.122321	332525.026345	41.961178
3505.050897	332458.428092	41.966183
3505.119549	332408.161392	41.971188
3504.894577	332345.198464	41.976192
3504.737156	332285.785534	41.981197
3504.848096	332233.782527	41.986202
3504.996531	332174.804840	41.991207
3505.093209	332128.653597	41.996212
3505.101338	332068.629478	42.001216
3505.042113	331999.434303	42.006221
3504.603304	331945.583903	42.011226
3504.920395	331889.377097	42.016231
3505.025763	331832.821805	42.021236
3504.802937	331779.522378	42.026240
3505.031180	331708.297909	42.031245
3504.546254	331660.354933	42.036250
3504.439212	331598.720324	42.041255
3504.763821	331543.173112	42.046260
3504.361917	331500.100246	42.051264
3504.620853	331445.097271	42.056269
3504.377237	331403.729053	42.061274
3504.527446	331357.771982	42.066279
3504.097613	331312.134445	42.071284
3504.050152	331256.034572	42.076288
3503.968941	331209.884598	42.081293
3504.020091	331160.610921	42.086298
3504.028704	331117.931259	42.091303
3504.383141	331074.230988	42.096308
3504.348926	331036.110638	42.101312
3504.403198	330978.849920	42.106317
3503.983628	330933.617275	42.111322
3503.873306	330878.544048	42.116327
3504.099219	330839.009386	42.121332
3504.334825	330801.889425	42.126336
3504.120906	330756.064867	42.131341
3504.279687	330705.171418	42.136346
3504.071427	330666.340316	42.141351
3503.904877	330625.188123	42.146356
3503.487043	330586.949262	42.151360
3503.598984	330544.278246	42.156365
3503.629043	330502.306716	42.161370
3503.839019	330466.741945	42.166375
3504.016534	330418.490380	42.171380
3503.878804	330384.226186	42.176384
3504.056221	330337.042787	42.181389
3504.020688	330296.327584	42.186394
3503.839851	330254.973754	42.191399
3504.055381	330207.428153	42.196404
3503.336444	330173.203768	42.201408
3503.580005	330128.019116	42.206413
3503.333176	330108.778226	42.211418
3503.517526	330075.633404	42.216423
3503.388139	330042.995429	42.221428
3503.226242	330001.256845	42.226432
3503.441377	329972.812564	42.231437
3503.455441	329945.391657	42.236442
3503.232166	329903.459085	42.241447
3503.679256	329871.519322	42.246452
3503.208839	329847.760410	42.251456
3503.676107	329795.520360	42.256461
3503.942115	329760.378578	42.261466
3503.523422	329722.113563	42.266471
3503.695871	329689.224623	42.271476
3503.396135	329646.744159	42.276480
3503.494964	329605.880052	42.281485
3503.454368	329584.012282	42.286490
3503.589467	329543.854622	42.291495
3503.460277	329515.184053	42.296500
3503.178256	329486.104958	42.301504
3503.334198	329437.397717	42.306509
3503.436177	329419.882418	42.311514
3503.656406	329382.992424	42.316519
3503.484400	329343.162358	42.321524
3503.339164	329316.935936	42.326528
3503.489546	329275.859942	42.331533
3503.095311	329249.723273	42.336538
3503.248215	329216.684380	42.341543
3503.151221	329180.301626	42.346548
3503.049117	329155.009459	42.351552
3503.040691	329131.584849	42.356557
3502.761536	329097.646859	42.361562
3502.765862	329078.366195	42.366567
3503.168953	329047.221137	42.371572
3502.883146	329026.586857	42.376576
3503.391227	328991.253927	42.381581
3503.296194	328957.922916	42.386586
3503.294193	328937.345962	42.391591
3503.152395	328899.011417	42.396596
3502.807844	328870.297738	42.401600
3502.990104	328840.458819	42.406605
3503.165680	328825.729661	42.411610
3503.113870	328793.154821	42.416615
3503.189982	328760.229292	42.421620
3502.972218	328738.668541	42.426624
3503.151605	328711.958557	42.431629
3503.472357	328682.428530	42.436634
3502.847866	328642.439573	42.441639
3503.148165	328616.321078	42.446644
3503.196125	328589.122843	42.451648
3503.031575	328565.773176	42.456653
3503.203962	328542.599741	42.461658
3503.253212	328511.077171	42.466663
3503.326298	328471.996414	42.471668
3502.909072	328446.498699	42.476672
3503.255559	328416.074196	42.481677
3503.225715	328389.269525	42.486682
3503.460217	328355.225154	42.491687
3503.599367	328317.431146	42.496692
3503.086783	328289.938801	42.501696
3503.424228	328259.286668	42.506701
3503.120092	328225.606190	42.511706
3503.252241	328197.453393	42.516711
3503.180063	328173.351409	42.521716
3502.983236	328141.307423	42.526720
3503.097113	328098.251900	42.531725
3503.193820	328086.917792	42.536730
3502.995413	328057.163230	42.541735
3503.185289	328026.915529	42.546740
3503.121630	328000.599168	42.551744
3503.273927	327963.540414	42.556749
3503.025286	327936.591590	42.561754
3502.984020	327910.831264	42.566759
3503.020994	327896.886514	42.571764
3502.966809	327869.932681	42.576768
3503.078887	327832.218751	42.581773
3502.978590	327809.418189	42.586778
3503.038897	327784.557606	42.591783
3502.805474	327753.332988	42.596788
3502.527992	327720.411002	42.601792
3502.791008	327703.454799	42.606797
3503.054059	327675.967948	42.611802
3502.879802	327652.848186	42.616807
3502.944486	327628.826220	42.621812
3502.664224	327599.720021	42.626816
3502.957392	327580.011924	42.631821
3502.852986	327555.838295	42.636826
3502.627901	327543.689503	42.641831
3502.566267	327520.297693	42.646836
3502.811478	327492.737195	42.651840
3503.088859	327463.620025	42.656845
3502.924848	327440.066119	42.661850
3502.661444	327409.507267	42.666855
3502.854989	327391.976753	42.671860
3502.501629	327366.061374	42.676864
3502.783883	327352.485072	42.681869
3502.682355	327329.531808	42.686874
3502.691674	327308.112832	42.691879
3503.225970	327283.126960	42.696884
3502.658644	327265.715344	42.701888
3502.781025	327235.299538	42.706893
3502.635077	327216.601067	42.711898
3502.543986	327196.316939	42.716903
3502.777916	327179.110695	42.721908
3502.900003	327161.489506	42.726912
3502.697717	327117.693815	42.731917
3502.975571	327100.709600	42.736922
3502.297004	327079.067367	42.741927
3502.589972	327054.526069	42.746932
3502.321013	327048.158119	42.751936
3502.680220	327017.577939	42.756941
3502.732096	327006.962761	42.761946
3502.453881	326976.380456	42.766951
3502.688975	326964.693716	42.771956
3502.510743	326932.086241	42.776960
3502.468539	326921.282255	42.781965
3502.168290	326902.506012	42.786970
3502.440937	326885.471647	42.791975
3502.685753	326874.393844	42.796980
3502.708372	326843.815280	42.801985
3502.795907	326825.537987	42.806989
3502.533705	326803.041967	42.811994
3502.533126	326782.234742	42.816999
3502.460789	326756.707460	42.822004
3502.280771	326751.215850	42.827009
3502.836492	326719.129379	42.832013
3502.714243	326700.121718	42.837018
3502.590103	326685.769307	42.842023
3502.639996	326666.912776	42.847028
3502.320606	326655.897684	42.852033
3502.847219	326634.066794	42.857037
3502.714984	326609.744321	42.862042
3502.924465	326594.347676	42.867047
3502.690105	326565.869473	42.872052
3502.672445	326551.322307	42.877057
3502.666052	326522.961056	42.882061
3502.520438	326500.980818	42.887066
3502.419850	326488.354374	42.892071
3502.833146	326462.954480	42.897076
3502.307508	326444.136948	42.902081
3502.392440	326419.729535	42.907085
3502.466999	326408.220354	42.912090
3502.538573	326381.754599	42.917095
3502.457532	326366.657658	42.922100
3502.015282	326354.593330	42.927105
3502.334843	326329.182568	42.932109
3502.228400	326323.908332	42.937114
3502.394950	326303.685222	42.942119
3502.602924	326283.455627	42.947124
3502.899854	326264.941845	42.952129
3502.974052	326249.795154	42.957133
3502.660164	326229.519932	42.962138
3502.374762	326197.615421	42.967143
3502.463823	326188.495013	42.972148
3502.592630	326167.896178	42.977153
3502.873637	326150.707571	42.982157
3502.830428	326132.323218	42.987162
3502.456940	326107.427664	42.992167
3502.788493	326078.962392	42.997172
3502.475504	326068.225948	43.002177
3502.622780	326032.488936	43.007181
3502.671754	326014.598864	43.012186
3502.571559	325997.698726	43.017191
3502.768271	325967.728214	43.022196
3502.217166	325961.480514	43.027201
3502.407792	325945.425196	43.032205
3502.456530	325941.958143	43.037210
3502.441153	325914.996927	43.042215
3502.231706	325903.837253	43.047220
3502.377055	325879.801630	43.052225
3502.356018	325858.055940	43.057229
3502.323157	325858.213758	43.062234
3502.401829	325833.247345	43.067239
3502.477275	325812.987359	43.072244
3502.043472	325793.620979	43.077249
3502.317312	325776.814897	43.082253
3502.167973	325765.772975	43.087258
3502.218319	325763.450344	43.092263
3502.658289	325725.683174	43.097268
3502.132704	325722.458516	43.102273
3502.062698	325705.350036	43.107277
3502.189885	325687.116903	43.112282
3502.169987	325677.046786	43.117287
3502.309226	325654.767179	43.122292
3502.309618	325642.480809	43.127297
3502.313658	325628.133419	43.132301
3502.396507	325614.867521	43.137306
3502.578899	325598.711604	43.142311
3502.411609	325585.204988	43.147316
3502.672843	325562.219441	43.152321
3502.599417	325549.334081	43.157325
3502.669630	325519.484765	43.162330
3502.785913	325512.598465	43.167335
3502.791324	325476.323513	43.172340
3502.466563	325465.588749	43.177345
3502.709541	325434.643977	43.182349
3502.635289	325426.897130	43.187354
3502.737311	325397.958511	43.192359
3502.620272	325376.380199	43.197364
3502.271131	325365.572907	43.202369
3502.318724	325339.110220	43.207373
3502.586776	325327.773984	43.212378
3502.383713	325312.568538	43.217383
3502.579480	325293.205243	43.222388
3502.252590	325272.778948	43.227393
3502.450047	325252.652235	43.232397
3502.303430	325242.271130	43.237402
3502.352122	325227.560487	43.242407
3502.554634	325207.789092	43.247412
3502.564854	325193.287955	43.252417
3502.501605	325179.230744	43.257421
3502.480142	325166.184511	43.262426
3502.545372	325137.582152	43.267431
3502.581166	325117.277143	43.272436
3502.300371	325107.552928	43.277441
3502.503059	325090.045425	43.282445
3502.517282	325066.665771	43.287450
3502.003510	325057.257785	43.292455
3502.234760	325043.663245	43.297460
3502.144290	325027.371694	43.302465
3502.525863	324997.397004	43.307469
3502.546166	324989.762482	43.312474
3502.326190	324975.246380	43.317479
3502.501566	324955.682609	43.322484
3502.697710	324937.311171	43.327489
3502.558924	324916.499156	43.332493
3502.822619	324896.438227	43.337498
3502.564867	324879.867513	43.342503
3502.298570	324855.971956	43.347508
3502.158027	324847.395905	43.352513
3502.412582	324822.070680	43.357517
3502.307029	324805.425265	43.362522
3502.553141	324803.962308	43.367527
3502.724094	324778.421183	43.372532
3502.546120	324764.483517	43.377537
3502.877675	324733.397176	43.382541
3501.976480	324717.537507	43.387546
3502.378653	324697.810965	43.392551
3502.689670	324674.664507	43.397556
3502.164029	324669.811727	43.402561
3502.516101	324654.366617	43.407565
3502.358665	324638.594145	43.412570
3502.369736	324618.903272	43.417575
3502.516418	324600.920989	43.422580
3502.395746	324590.968112	43.427585
3501.993558	324572.028657	43.432589
3502.361412	324552.053028	43.437594
3502.547981	324531.902225	43.442599
3502.168720	324518.555587	43.447604
3502.127215	324502.866692	43.452609
3502.384004	324484.409254	43.457613
3502.227185	324475.250588	43.462618
3502.318654	324465.671528	43.467623
3502.458781	324444.230587	43.472628
3502.482740	324433.644540	43.477633
3502.309713	324406.325399	43.482637
3502.567532	324401.502732	43.487642
3502.137511	324371.959730	43.492647
3502.355980	324353.406471	43.497652
3502.126028	324354.485452	43.502657
3502.577160	324321.421346	43.507661
3502.579675	324323.201698	43.512666
3502.372961	324305.706990	43.517671
3502.687194	324288.334337	43.522676
3502.464583	324272.114021	43.527681
3502.493586	324247.078089	43.532685
3502.889549	324226.690892	43.537690
3502.760985	324202.875176	43.542695
3502.810521	324187.349997	43.547700
3502.482795	324163.361886	43.552705
3502.262876	324137.398139	43.557709
3502.325475	324127.136673	43.562714
3502.216188	324116.215236	43.567719
3502.167341	324102.129965	43.572724
3502.002116	324075.776050	43.577729
3502.037263	324069.843420	43.582733
3502.021206	324067.785460	43.587738
3502.209432	324045.192056	43.592743
3502.427472	324024.883453	43.597748
3502.269545	324024.043285	43.602753
3501.981949	323997.403188	43.607757
3502.068817	323982.202797	43.612762
3502.333751	323973.614049	43.617767
3502.457258	323958.382483	43.622772
3502.134490	323945.408406	43.627777
3502.204147	323939.343169	43.632781
3502.277906	323917.225486	43.637786
3501.995753	323907.602953	43.642791
3502.461871	323895.141495	43.647796
3502.084250	323881.132987	43.652801
3501.899048	323865.084733	43.657805
3501.981977	323852.530537	43.662810
3501.895836	323853.739679	43.667815
3501.860292	323837.464508	43.672820
3501.938741	323820.789928	43.677825
3502.044531	323806.985645	43.682829
3502.231339	323804.667007	43.687834
3502.292410	323800.078540	43.692839
3502.387921	323775.438944	43.697844
3501.835955	323770.920876	43.702849
3502.059850	323758.955143	43.707853
3502.071403	323734.811985	43.712858
3502.060111	323718.863680	43.717863
3502.333870	323707.449790	43.722868
3501.880625	323699.939939	43.727873
3501.814387	323682.270371	43.732877
3502.289550	323670.901300	43.737882
3502.057920	323678.823605	43.742887
3502.251691	323651.243108	43.747892
3501.965244	323644.979113	43.752897
3502.082133	323636.006419	43.757901
3502.032129	323624.236101	43.762906
3501.707743	323604.037533	43.767911
3501.995860	323591.807323	43.772916
3501.811358	323580.465042	43.777921
3502.110702	323588.507863	43.782925
3501.998169	323586.693912	43.787930
3502.233331	323567.018380	43.792935
3502.247333	323545.825641	43.797940
3502.178123	323544.564571	43.802945
3502.176027	323522.433098	43.807949
3502.061520	323501.896401	43.812954
3501.890185	323492.994175	43.817959
3502.180593	323479.669699	43.822964
3501.932528	323469.889101	43.827969
3502.192674	323460.410632	43.832973
3502.304626	323457.823850	43.837978
3502.146728	323438.616731	43.842983
3502.176966	323420.703018	43.847988
3502.047823	323411.997690	43.852993
3501.982751	323403.333222	43.857997
3502.123449	323386.852248	43.863002
3501.976101	323376.190955	43.868007
3501.719204	323367.505591	43.873012
3502.018925	323370.435154	43.878017
3502.107566	323346.457791	43.883021
3502.030378	323332.376689	43.888026
3502.003535	323330.091427	43.893031
3502.433074	323316.668831	43.898036
3502.064921	323294.187439	43.903041
3502.068757	323286.351663	43.908045
3501.950600	323292.297493	43.913050
3501.789209	323268.740762	43.918055
3501.980643	323256.296616	43.923060
3502.436212	323248.364771	43.928065
3502.381219	323233.491553	43.933069
3502.358417	323218.765932	43.938074
3501.782766	323214.531335	43.943079
3502.012812	323207.703182	43.948084
3501.951775	323197.944158	43.953089
3501.940881	323166.375955	43.958093
3501.837418	323162.118410	43.963098
3501.705447	323170.406818	43.968103
3502.154304	323158.456621	43.973108
3502.205748	323148.705440	43.978113
3501.954472	323125.289875	43.983117
3502.025413	323122.760362	43.988122
3501.980870	323110.531140	43.993127
3502.182848	323085.721855	43.998132
3501.889784	323079.611443	44.003137
3501.842576	323070.969552	44.008141
3501.742507	323062.539437	44.013146
3501.538345	323063.487222	44.018151
3501.713649	323042.319887	44.023156
3501.748006	323040.584705	44.028161
3501.618774	323032.057386	44.033165
3501.645862	323030.908441	44.038170
3501.504105	323032.609648	44.043175
3501.755115	323028.322110	44.048180
3501.418949	323028.196646	44.053185
3501.644839	323024.447259	44.058189
3502.137267	323023.886984	44.063194
3501.861823	323001.721650	44.068199
3501.942503	322984.944629	44.073204
3501.687044	322989.080341	44.078209
3501.654068	322979.876543	44.083213
3501.900012	322975.259082	44.088218
3501.781941	322954.875307	44.093223
3501.943159	322941.825250	44.098228
3502.045694	322938.018822	44.103233
3501.664950	322944.209268	44.108237
3501.622503	322926.917249	44.113242
3501.957749	322930.299196	44.118247
3501.812623	322904.730012	44.123252
3501.757960	322901.406064	44.128257
3501.589300	322894.131407	44.133261
3502.127824	322898.168438	44.138266
3501.747753	322889.934699	44.143271
3501.750691	322866.453806	44.148276
3501.687934	322853.158905	44.153281
3501.748918	322855.718798	44.158285
3501.733224	322854.678294	44.163290
3502.013339	322854.965268	44.168295
3502.200135	322846.566579	44.173300
3501.859649	322828.049147	44.178305
3502.115394	322811.677156	44.183309
3501.943517	322808.218890	44.188314
3501.851601	322805.282349	44.193319
3502.023989	322779.485373	44.198324
3502.073819	322776.450353	44.203329
3501.975415	322761.202162	44.208333
3502.137336	322769.419264	44.213338
3502.083410	322755.029057	44.218343
3502.282057	322734.264947	44.223348
3502.002212	322730.492842	44.228353
3502.092094	322724.958494	44.233357
3502.094065	322699.925855	44.238362
3502.007131	322692.256794	44.243367
3502.293589	322685.089024	44.248372
3502.207615	322679.861997	44.253377
3502.233118	322648.745622	44.258381
3502.052413	322653.353030	44.263386
3501.980722	322641.356870	44.268391
3501.956874	322606.050668	44.273396
3501.735295	322613.055782	44.278401
3501.953523	322604.575813	44.283405
3501.881697	322612.905807	44.288410
3501.686780	322588.387232	44.293415
3502.146971	322579.055366	44.298420
3501.662254	322567.352712	44.303425
3501.946303	322564.128421	44.308429
3502.224864	322554.443352	44.313434
3501.792994	322542.554352	44.318439
3501.921924	322526.939822	44.323444
3501.637433	322531.588909	44.328449
3501.739415	322524.526271	44.333453
3502.044546	322520.993406	44.338458
3501.696296	322513.645002	44.343463
3501.837472	322497.952227	44.348468
3501.808699	322484.702775	44.353473
3501.707424	322482.174708	44.358477
3501.976776	322478.698312	44.363482
3501.751062	322484.381237	44.368487
3501.973639	322463.715010	44.373492
3501.568882	322449.048832	44.378497
3501.947371	322449.651144	44.383501
3502.438603	322447.997147	44.388506
3502.067997	322449.606957	44.393511
3502.371963	322417.887205	44.398516
3502.229819	322400.305279	44.403521
3501.963952	322386.889346	44.408525
3501.651500	322377.703668	44.413530
3501.748494	322367.538150	44.418535
3501.904311	322353.954522	44.423540
3501.923536	322358.937739	44.428545
3502.410564	322351.738556	44.433549
3502.096600	322327.263880	44.438554
3502.102119	322310.829054	44.443559
3502.093050	322314.849994	44.448564
3501.706974	322299.443092	44.453569
3501.658213	322290.419688	44.458573
3501.891643	322280.309137	44.463578
3501.339516	322270.016121	44.468583
3501.875209	322271.865843	44.473588
3501.455581	322271.244631	44.478593
3501.622320	322262.848961	44.483597
3501.873563	322268.559107	44.488602
3501.786603	322257.455613	44.493607
3501.946872	322234.967357	44.498612
3502.041749	322230.780467	44.503617
3501.756876	322226.602067	44.508621
3501.924143	322218.893178	44.513626
3501.807025	322218.402749	44.518631
3501.938650	322193.909212	44.523636
3501.959324	322182.916070	44.528641
3501.815534	322186.067693	44.533645
3502.089686	322183.455474	44.538650
3501.724624	322173.107748	44.543655
3502.369888	322146.778539	44.548660
3502.063559	322145.401859	44.553665
3501.849976	322138.159534	44.558669
3502.049804	322121.134581	44.563674
3501.595742	322117.008061	44.568679
3501.747092	322099.278365	44.573684
3501.600969	322108.841185	44.578689
3501.820720	322099.928399	44.583693
3501.865738	322096.054568	44.588698
3501.790902	322079.886613	44.593703
3502.284265	322053.911812	44.598708
3501.799855	322054.674474	44.603713
3501.654973	322047.802990	44.608717
3501.917177	322046.413742	44.613722
3502.185362	322036.552097	44.618727
3502.115654	322023.207140	44.623732
3501.923288	322011.026147	44.628737
3502.020516	322014.343621	44.633741
3501.891885	321992.409198	44.638746
3501.805923	321977.565816	44.643751
3502.030730	321962.902802	44.648756
3501.944316	321956.810797	44.653761
3501.677906	321961.050082	44.658765
3501.747729	321942.442670	44.663770
3501.360160	321931.767686	44.668775
3501.919320	321920.690289	44.673780
3501.776018	321927.225361	44.678785
3501.619503	321920.075835	44.683789
3502.093984	321911.810063	44.688794
3501.670288	321916.709939	44.693799
3501.980098	321890.738294	44.698804
3501.594185	321883.726386	44.703809
3501.507808	321880.178356	44.708813
3501.625445	321872.324524	44.713818
3501.532439	321888.137311	44.718823
3501.635317	321871.432693	44.723828
3501.709034	321870.327307	44.728833
3501.630028	321869.474757	44.733837
3501.980141	321861.431938	44.738842
3501.546373	321852.468631	44.743847
3502.109583	321847.241767	44.748852
3501.813151	321841.767698	44.753857
3501.706975	321842.064192	44.758861
3502.034591	321836.289041	44.763866
3501.576390	321820.384441	44.768871
3501.824225	321811.111044	44.773876
3501.716865	321800.697498	44.778881
3501.781713	321804.249011	44.783885
3502.004305	321790.527562	44.788890
3501.875901	321796.042726	44.793895
3501.886634	321775.282081	44.798900
3502.061531	321761.033839	44.803905
3502.050119	321762.765598	44.808909
3501.978818	321761.326721	44.813914
3502.043510	321739.031223	44.818919
3502.089579	321722.589829	44.823924
3501.908024	321726.281630	44.828929
3501.905597	321720.507182	44.833933
3501.669496	321710.342701	44.838938
3501.930329	321693.384359	44.843943
3501.930658	321677.738739	44.848948
3501.834161	321676.990679	44.853953
3502.013962	321664.268041	44.858957
3502.183781	321653.200563	44.863962
3501.927142	321641.385673	44.868967
3502.154378	321631.454016	44.873972
3502.079696	321634.162394	44.878977
3501.866389	321615.904384	44.883981
3502.037850	321589.343621	44.888986
3501.745923	321587.939231	44.893991
3501.664257	321588.918777	44.898996
3501.635595	321590.271638	44.904001
3502.052648	321572.169461	44.909005
3502.115847	321558.091254	44.914010
3502.021631	321557.139315	44.919015
3501.257875	321545.454559	44.924020
3501.348739	321544.931607	44.929025
3501.507525	321539.360890	44.934029
3501.510306	321537.121780	44.939034
3501.675490	321550.146794	44.944039
3501.564463	321540.089918	44.949044
3501.562708	321541.692976	44.954049
3501.427099	321531.970663	44.959053
3501.728875	321504.626270	44.964058
3501.380835	321510.811813	44.969063
3501.728232	321509.943472	44.974068
3501.564969	321508.442643	44.979073
3501.438050	321500.525214	44.984077
3501.696907	321502.341931	44.989082
3501.553098	321507.274418	44.994087
3501.428408	321495.769579	44.999092
3501.637919	321497.746652	45.004097
3501.673102	321503.948603	45.009101
3501.855104	321492.930059	45.014106
3501.725931	321476.439646	45.019111
3501.679132	321464.362938	45.024116
3501.587228	321464.021199	45.029121
3501.541849	321460.441285	45.034125
3501.537628	321458.254145	45.039130
3501.652593	321461.848732	45.044135
3502.006112	321449.607674	45.049140
3501.429407	321459.695880	45.054145
3501.427140	321445.755072	45.059149
3501.476395	321430.788597	45.064154
3501.246492	321421.309962	45.069159
3501.360933	321412.871420	45.074164
3501.395481	321423.830799	45.079169
3501.604707	321422.017331	45.084173
3501.741689	321415.585041	45.089178
3501.599134	321410.163180	45.094183
3501.547746	321408.136052	45.099188
3502.037756	321412.409775	45.104193
3501.667272	321412.035268	45.109197
3501.611785	321407.744603	45.114202
3501.708849	321414.878181	45.119207
3501.664397	321396.364715	45.124212
3501.790628	321382.658200	45.129217
3501.695643	321375.397201	45.134221
3502.375266	321365.801800	45.139226
3501.958651	321371.362078	45.144231
3501.886235	321347.739477	45.149236
3501.780632	321337.300102	45.154241
3501.646135	321339.305523	45.159245
3501.587390	321322.346115	45.164250
3501.246947	321320.313294	45.169255
3501.666044	321316.431789	45.174260
3502.069972	321319.345205	45.179265
3501.770664	321325.726678	45.184269
3501.963781	321301.197569	45.189274
3501.919691	321289.807275	45.194279
3502.038470	321288.389546	45.199284
3501.700867	321291.139051	45.204289
3501.724931	321281.213635	45.209293
3501.834904	321255.552687	45.214298
3501.724905	321252.160939	45.219303
3501.979394	321248.763088	45.224308
3501.809967	321257.846378	45.229313
3501.475011	321239.607224	45.234317
3501.843509	321240.134795	45.239322
3501.335883	321248.965676	45.244327
3501.694647	321236.698297	45.249332
3501.768094	321223.050862	45.254337
3501.623162	321210.175334	45.259341
3501.950286	321209.742642	45.264346
3501.710396	321210.645173	45.269351
3502.135702	321197.833132	45.274356
3501.979805	321191.192193	45.279361
3502.258984	321185.500847	45.284365
3501.820142	321170.992194	45.289370
3501.871679	321181.109449	45.294375
3501.765990	321162.122089	45.299380
3501.798191	321150.745271	45.304385
3502.082501	321129.559934	45.309389
3501.969163	321118.892750	45.314394
3501.976664	321132.502233	45.319399
3502.161568	321103.471349	45.324404
3502.151748	321099.402477	45.329409
3502.113344	321082.745078	45.334413
3502.065166	321075.171426	45.339418
3501.654138	321063.456832	45.344423
3502.420628	321056.264620	45.349428
3502.013777	321040.555221	45.354433
3501.941442	321040.312181	45.359437
3501.968190	321015.427311	45.364442
3501.921148	321016.045292	45.369447
3501.898419	321009.892314	45.374452
3502.098307	321001.465771	45.379457
3501.909892	320973.536221	45.384461
3502.138876	320964.469111	45.389466
3501.718609	320970.360738	45.394471
3501.844768	320967.262773	45.399476
3501.735011	320957.281882	45.404481
3501.740249	320944.026629	45.409485
3501.558144	320932.250769	45.414490
3501.695333	320926.276301	45.419495
3501.922061	320920.847525	45.424500
3501.667421	320924.220096	45.429505
3501.543806	320918.413603	45.434509
3501.954525	320919.952198	45.439514
3501.657675	320903.106169	45.444519
3501.695675	320892.338948	45.449524
3501.972795	320888.148875	45.454529
3501.791872	320876.627219	45.459533
3502.097456	320877.419037	45.464538
3501.919748	320871.671876	45.469543
3502.144094	320850.953705	45.474548
3502.136931	320834.596611	45.479553
3501.840685	320833.981527	45.484557
3502.350912	320823.979999	45.489562
3501.841809	320806.989031	45.494567
3501.478102	320798.294393	45.499572
3501.595830	320787.641883	45.504577
3501.795816	320793.843614	45.509581
3502.023005	320784.878509	45.514586
3501.642062	320779.264871	45.519591
3501.932103	320757.951250	45.524596
3502.036782	320761.191336	45.529601
3501.550139	320751.600047	45.534605
3502.110611	320748.357844	45.539610
3501.560457	320749.817702	45.544615
3501.797189	320719.150256	45.549620
3501.881333	320715.499147	45.554625
3501.808053	320712.788513	45.559629
3501.881244	320705.755514	45.564634
3501.608007	320714.931470	45.569639
3501.735313	320706.923267	45.574644
3501.848566	320686.909281	45.579649
3501.609437	320679.314530	45.584653
3501.563935	320670.748202	45.589658
3501.744934	320668.710150	45.594663
3501.864623	320667.215935	45.599668
3501.653482	320670.785250	45.604673
3501.530120	320667.090257	45.609677
3501.659418	320660.328326	45.614682
3501.897967	320647.825165	45.619687
3501.780832	320633.418677	45.624692
3501.345828	320632.163826	45.629697
3501.708540	320625.950533	45.634701
3501.468276	320619.755186	45.639706
3501.806873	320631.252370	45.644711
3501.775198	320626.423650	45.649716
3501.636315	320618.889538	45.654721
3501.619573	320612.099550	45.659725
3501.787375	320597.216011	45.664730
3501.539094	320593.973033	45.669735
3501.624773	320582.892991	45.674740
3501.573372	320577.405891	45.679745
3501.626787	320579.407411	45.684749
3501.894005	320574.964448	45.689754
3501.906927	320575.115128	45.694759
3501.471203	320563.963952	45.699764
3501.723067	320555.351112	45.704769
3501.727159	320553.976728	45.709773
3501.756442	320550.181539	45.714778
3501.627027	320549.871098	45.719783
3501.602578	320549.773212	45.724788
3501.769938	320536.645131	45.729793
3501.570031	320533.445467	45.734797
3501.837174	320532.640536	45.739802
3501.598373	320517.413486	45.744807
3501.842321	320508.064092	45.749812
3501.544070	320512.333938	45.754817
3501.604311	320496.322347	45.759821
3501.804593	320439.151129	45.764826
3501.578446	320343.681733	45.769831
3501.793678	320199.932593	45.774836
3501.205915	320001.941038	45.779841
3501.268746	319762.759366	45.784845
3500.725282	319472.686711	45.789850
3500.614428	319150.996975	45.794855
3500.602255	318755.762763	45.799860
3499.888170	318336.083163	45.804865
3499.606488	317859.035928	45.809869
3499.251464	317332.483722	45.814874
3498.703685	316756.341706	45.819879
3498.261851	316138.346944	45.824884
3498.080426	315469.517444	45.829889
3497.386327	314764.882098	45.834893
3497.085222	314002.339152	45.839898
3496.285586	313201.872243	45.844903
3495.446449	312334.807146	45.849908
3495.195972	311440.508667	45.854913
3494.071983	310485.742047	45.859917
3493.413611	309476.910692	45.864922
3492.296815	308445.888917	45.869927
3491.864477	307351.220226	45.874932
3490.921869	306209.018327	45.879937
3489.727805	305024.813239	45.884941
3488.679405	303788.207722	45.889946
3487.840018	302507.638112	45.894951
3486.953093	301199.226882	45.899956
3486.072898	299821.579595	45.904961
3484.697591	298403.633056	45.909965
3483.666375	296931.381760	45.914970
3482.528512	295421.361248	45.919975
3480.973481	293864.276188	45.924980
3479.656982	292271.323290	45.929985
3478.093759	290641.787441	45.934989
3476.947850	288964.922214	45.939994
3475.765727	287250.673251	45.944999
3473.831465	285471.503663	45.950004
3472.507509	283681.830371	45.955009
3471.041457	281844.244960	45.960013
3469.027335	279969.552701	45.965018
3467.393584	278055.137547	45.970023
3466.003341	276093.126712	45.975028
3463.899738	274101.211141	45.980033
3462.035958	272061.239774	45.985037
3460.433082	269995.538834	45.990042
3458.613850	267894.507229	45.995047
3456.816101	265760.170238	46.000052
3454.733836	263588.246953	46.005057
3452.508758	261376.907346	46.010061
3450.811027	259130.808945	46.015066
3448.601018	256873.823841	46.020071
3446.662112	254562.844550	46.025076
3444.520527	252225.856965	46.030081
3441.860667	249849.083623	46.035085
3440.043523	247447.389994	46.040090
3437.332564	245015.294211	46.045095
3434.824498	242556.676610	46.050100
3432.829748	240065.990235	46.055105
3430.285930	237550.993657	46.060109
3427.733864	235007.301376	46.065114
3425.015092	232435.476444	46.070119
3422.376212	229836.477299	46.075124
3419.836691	227215.806195	46.080129
3417.248154	224572.166198	46.085133
3414.336913	221895.213219	46.090138
3411.096746	219217.476898	46.095143
3408.417547	216509.864743	46.100148
3405.426627	213787.977957	46.105153
3402.282985	211037.967533	46.110157
3399.503295	208276.491089	46.115162
3396.056717	205490.522952	46.120167
3392.978454	202685.230180	46.125172
3389.931028	199868.108156	46.130177
3386.088420	197037.483953	46.135181
3382.754351	194196.343297	46.140186
3379.747343	191356.460413	46.145191
3376.232407	188487.999206	46.150196
3372.736086	185624.345202	46.155201
3368.573829	182747.659055	46.160205
3365.599952	179855.366161	46.165210
3361.555290	176966.134166	46.170215
3357.881153	174067.000141	46.175220
3354.051483	171159.466377	46.180225
3350.164839	168261.600313	46.185229
3345.926476	165351.406296	46.190234
3341.541798	162459.751650	46.195239
3337.412318	159566.683517	46.200244
3332.752288	156698.498079	46.205249
3327.824495	153827.908865	46.210253
3323.275191	150959.300542	46.215258
3318.276633	148122.076189	46.220263
3313.274146	145286.111353	46.225268
3308.058639	142499.464084	46.230273
3302.310024	139639.479412	46.235277
3296.851337	136890.661755	46.240282
3290.851612	134195.930101	46.245287
3284.488034	131551.931840	46.250292
3277.976391	128934.664012	46.255297
3270.950800	126381.972506	46.260301
3264.083192	123871.779626	46.265306
3256.904168	121421.705345	46.270311
3249.087612	119058.956698	46.275316
3241.533001	116740.653877	46.280321
3233.189132	114516.419313	46.285325
3224.850891	112376.616712	46.290330
3216.062356	110329.543608	46.295335
3207.642616	108367.417483	46.300340
3198.949841	106506.522200	46.305345
3189.558039	104750.316454	46.310349
3180.871969	103073.549908	46.315354
3171.537052	101526.529224	46.320359
3162.508945	100064.729309	46.325364
3153.311632	98713.340849	46.330369
3144.601382	97461.597770	46.335373
3136.436566	96298.779057	46.340378
3128.232298	95237.306457	46.345383
3120.452300	94251.974123	46.350388
3113.551560	93367.102229	46.355393
3106.622333	92544.042133	46.360397
3100.527994	91786.402507	46.365402
3094.195747	91092.605558	46.370407
3087.958204	90446.419941	46.375412
3082.444298	89862.610327	46.380417
3077.252296	89328.581008	46.385421
3072.186705	88830.790395	46.390426
3066.961026	88382.914359	46.395431
3062.308346	87951.370572	46.400436
3058.235680	87563.803331	46.405441
3053.774500	87188.028518	46.410445
3050.042238	86838.417828	46.415450
3046.340753	86499.579953	46.420455
3042.259090	86176.749491	46.425460
3039.076165	85874.299462	46.430465
3036.029428	85568.312229	46.435469
3032.613203	85265.638229	46.440474
3029.142325	84978.461974	46.445479
3026.471082	84684.481344	46.450484
3023.026987	84391.780599	46.455489
3019.728250	84096.328845	46.460493
3016.569858	83800.311938	46.465498
3013.511350	83512.463353	46.470503
3009.952697	83218.877852	46.475508
3006.915658	82925.683809	46.480513
3003.634361	82636.748328	46.485517
3000.766598	82340.840831	46.490522
2996.964890	82045.133285	46.495527
2993.775741	81753.956728	46.500532
2990.377414	81454.305325	46.505537
2986.654158	81155.114392	46.510541
2983.497454	80865.453497	46.515546
2979.962500	80572.476031	46.520551
2976.314177	80275.086434	46.525556
2973.037236	79983.649804	46.530561
2969.303864	79696.631522	46.535565
2965.926161	79406.982193	46.540570
2961.756988	79123.302242	46.545575
2958.275534	78824.060365	46.550580
2954.942921	78555.877793	46.555585
2950.741160	78283.921880	46.560589
2947.362004	78003.012980	46.565594
2943.808530	77746.595622	46.570599
2940.246562	77474.255544	46.575604
2936.619289	77216.165519	46.580609
2932.885702	76949.166267	46.585613
2929.178654	76678.774540	46.590618
2925.834246	76436.002126	46.595623
2922.119450	76179.624701	46.600628
2918.882069	75912.519911	46.605633
2914.931932	75669.874479	46.610637
2911.148852	75420.080647	46.615642
2907.629763	75170.031949	46.620647
2904.216147	74936.008317	46.625652
2900.758221	74689.027753	46.630657
2896.874072	74456.770875	46.635661
2893.422647	74203.990268	46.640666
2889.669183	73966.155050	46.645671
2886.229782	73734.761895	46.650676
2882.535701	73502.699451	46.655681
2879.024788	73279.867617	46.660685
2875.185263	73059.120792	46.665690
2871.639666	72819.002979	46.670695
2868.283896	72600.838257	46.675700
2864.504183	72372.100618	46.680705
2861.293095	72157.650164	46.685709
2857.926799	71925.245500	46.690714
2854.385543	71711.802648	46.695719
2850.557999	71493.212947	46.700724
2847.264811	71269.614830	46.705729
2843.375954	71056.612590	46.710733
2840.233002	70823.852593	46.715738
2836.732898	70606.044402	46.720743
2832.982278	70389.788167	46.725748
2829.957845	70167.935025	46.730753
2826.062668	69945.635895	46.735757
2822.994550	69731.424161	46.740762
2819.274537	69510.059970	46.745767
2816.231225	69283.798857	46.750772
2812.565474	69063.623470	46.755777
2809.764682	68835.557177	46.760781
2806.129004	68614.542948	46.765786
2802.239772	68383.864041	46.770791
2799.108348	68148.428267	46.775796
2796.118046	67920.996410	46.780801
2791.876316	67692.048355	46.785805
2788.832412	67467.790158	46.790810
2784.991228	67251.993292	46.795815
2781.644892	67003.899667	46.800820
2778.432246	66782.136796	46.805825
2774.479723	66551.401759	46.810829
2771.249356	66306.242081	46.815834
2767.517078	66086.965919	46.820839
2763.849151	65859.855165	46.825844
2760.578021	65626.203682	46.830849
2757.057644	65395.208446	46.835853
2753.710556	65159.960922	46.840858
2750.038839	64930.504260	46.845863
2746.601440	64705.881318	46.850868
2743.093061	64469.611832	46.855873
2739.604973	64250.199175	46.860877
2736.282255	64009.341444	46.865882
2732.629848	63772.288633	46.870887
2729.614879	63543.173515	46.875892
2725.951899	63313.609678	46.880897
2722.269474	63090.937234	46.885901
2718.952194	62840.639581	46.890906
2715.452916	62609.698431	46.895911
2711.801278	62368.381209	46.900916
2708.602230	62132.916848	46.905921
2704.831245	61903.903337	46.910925
2701.441409	61660.356187	46.915930
2697.948229	61421.295424	46.920935
2694.326874	61180.822768	46.925940
2690.730558	60954.652917	46.930945
2687.499832	60712.010452	46.935949
2683.867467	60475.696800	46.940954
2680.627888	60245.771561	46.945959
2677.047160	60005.405597	46.950964
2673.635636	59762.756387	46.955969
2670.039090	59527.360104	46.960973
2666.673690	59288.198616	46.965978
2663.302174	59050.093824	46.970983
2659.591160	58812.203109	46.975988
2656.065370	58564.278741	46.980993
2652.772867	58327.367999	46.985997
2649.285747	58075.260879	46.991002
2645.629870	57831.780811	46.996007
2642.081674	57600.507493	47.001012
2638.581952	57350.535607	47.006017
2635.106630	57111.780845	47.011021
2631.727910	56876.985413	47.016026
2628.034318	56635.788571	47.021031
2624.323455	56378.055373	47.026036
2621.172513	56144.627397	47.031041
2617.448622	55905.390564	47.036045
2614.271020	55653.457150	47.041050
2610.647188	55420.928709	47.046055
2607.371213	55169.802553	47.051060
2603.784215	54925.909832	47.056065
2600.162880	54682.253396	47.061069
2596.340372	54440.109206	47.066074
2593.184054	54190.104037	47.071079
2589.595679	53948.600773	47.076084
2586.074843	53699.285916	47.081089
2582.148587	53465.136420	47.086093
2579.182774	53214.236299	47.091098
2575.371410	52961.009606	47.096103
2571.852609	52725.046442	47.101108
2568.736598	52481.105362	47.106113
2565.053021	52241.271306	47.111117
2561.589494	51993.608702	47.116122
2558.533655	51743.315726	47.121127
2554.741667	51491.167697	47.126132
2551.410068	51248.123301	47.131137
2547.746825	50999.056178	47.136141
2544.693823	50739.175745	47.141146
2540.892739	50494.461885	47.146151
2537.600165	50246.708720	47.151156
2534.109236	49994.929527	47.156161
2530.540454	49744.110407	47.161165
2526.972354	49488.149609	47.166170
2523.345771	49242.134098	47.171175
2519.827400	48972.425786	47.176180
2516.594668	48724.102455	47.181185
2512.584081	48481.301294	47.186189
2508.889228	48230.505776	47.191194
2505.758161	47976.998929	47.196199
2502.362352	47723.035244	47.201204
2498.826425	47480.069024	47.206209
2495.104703	47229.301432	47.211213
2491.888199	46974.912145	47.216218
2488.128229	46727.600050	47.221223
2484.643190	46463.161428	47.226228
2481.502125	46214.800443	47.231233
2477.959603	45959.737883	47.236237
2474.381139	45712.934924	47.241242
2470.812502	45452.675325	47.246247
2467.382948	45194.965484	47.251252
2464.311121	44945.275879	47.256257
2460.163309	44687.589107	47.261261
2456.849562	44425.430736	47.266266
2453.069940	44184.478793	47.271271
2450.051570	43927.188532	47.276276
2446.565473	43667.932439	47.281281
2442.643482	43423.313899	47.286285
2439.386364	43148.212447	47.291290
2436.111144	42908.121286	47.296295
2432.329078	42642.487047	47.301300
2429.106278	42380.604919	47.306305
2425.724732	42129.340357	47.311309
2422.350121	41863.886373	47.316314
2418.843253	41602.051596	47.321319
2415.170834	41334.126901	47.326324
2411.532981	41076.548242	47.331329
2408.171443	40816.646728	47.336333
2404.812809	40554.084779	47.341338
2401.424595	40283.167412	47.346343
2397.589493	40031.712525	47.351348
2394.136057	39758.827306	47.356353
2390.619331	39506.865830	47.361357
2387.479341	39237.216079	47.366362
2384.025247	38974.669098	47.371367
2380.266296	38705.966032	47.376372
2377.061637	38431.169251	47.381377
2373.153478	38170.281738	47.386381
2369.497297	37895.410259	47.391386
2366.055192	37645.056457	47.396391
2362.219179	37372.945899	47.401396
2359.242046	37113.973278	47.406401
2355.394649	36863.159473	47.411405
2352.051498	36577.922415	47.416410
2348.687088	36324.047142	47.421415
2345.267882	36055.488909	47.426420
2341.665765	35784.471354	47.431425
2338.388753	35525.615617	47.436429
2334.755964	35249.449601	47.441434
2331.186835	34982.614568	47.446439
2327.951099	34724.763704	47.451444
2324.369383	34447.376739	47.456449
2320.801789	34184.348501	47.461453
2317.523730	33899.676020	47.466458
2314.163138	33628.939850	47.471463
2310.411433	33362.692636	47.476468
2307.217714	33092.121089	47.481473
2303.470366	32827.388531	47.486477
2300.310436	32547.533039	47.491482
2296.836864	32272.819921	47.496487
2293.294720	31995.414773	47.501492
2289.936139	31709.352217	47.506497
2286.339764	31438.402394	47.511501
2282.731336	31151.391540	47.516506
2279.119444	30874.043943	47.521511
2275.417900	30587.657542	47.526516
2272.083958	30308.385405	47.531521
2268.518733	30038.608782	47.536525
2265.084368	29753.757499	47.541530
2261.696408	29475.430344	47.546535
2258.376023	29201.570478	47.551540
2255.075482	28916.728850	47.556545
2250.927297	28636.865316	47.561549
2247.610171	28359.017488	47.566554
2244.192072	28076.157729	47.571559
2240.820968	27796.462940	47.576564
2237.318429	27510.310074	47.581569
2233.807935	27241.493185	47.586573
2230.559848	26951.335290	47.591578
2226.924667	26661.837727	47.596583
2223.444259	26385.632806	47.601588
2219.567343	26101.668369	47.606593
2215.942556	25823.409071	47.611597
2212.502186	25535.519207	47.616602
2209.230096	25246.865809	47.621607
2205.793356	24971.877234	47.626612
2202.406172	24680.620550	47.631617
2198.400934	24406.393923	47.636621
2194.983702	24130.881611	47.641626
2191.287558	23852.458010	47.646631
2187.656656	23574.047086	47.651636
2184.023639	23294.804102	47.656641
2180.528117	23033.459801	47.661645
2177.022118	22752.487674	47.666650
2173.292436	22482.919765	47.671655
2169.312097	22215.941430	47.676660
2165.868985	21959.424042	47.681665
2161.817573	21694.155302	47.686669
2158.205835	21436.530798	47.691674
2154.573314	21193.324425	47.696679
2150.422152	20955.681679	47.701684
2146.530933	20723.550228	47.706689
2142.320113	20494.714795	47.711693
2138.593575	20266.065970	47.716698
2135.062596	20043.907276	47.721703
2130.851798	19823.301686	47.726708
2127.211452	19621.859045	47.731713
2123.513851	19417.729086	47.736717
2120.466928	19203.409240	47.741722
2116.506904	19002.257374	47.746727
2112.698992	18813.073984	47.751732
2109.557519	18608.092747	47.756737
2106.125804	18412.685173	47.761741
2102.695355	18213.998472	47.766746
2099.411665	18017.146620	47.771751
2096.058066	17829.054469	47.776756
2092.597397	17607.609263	47.781761
2088.756178	17429.243333	47.786765
2085.258523	17220.988395	47.791770
2082.170560	17023.698018	47.796775
2078.495061	16822.916930	47.801780
2074.786375	16636.703281	47.806785
2071.082009	16442.419101	47.811789
2068.091270	16236.375437	47.816794
2064.631135	16047.297700	47.821799
2061.313480	15842.591856	47.826804
2057.975347	15637.403764	47.831809
2054.232791	15445.250855	47.836813
2050.848762	15237.743733	47.841818
2047.316178	15040.524296	47.846823
2043.837436	14842.643041	47.851828
2040.316386	14641.645319	47.856833
2036.712097	14449.293986	47.861837
2033.511474	14247.743679	47.866842
2029.843163	14047.797961	47.871847
2026.568073	13853.463427	47.876852
2023.195985	13641.194070	47.881857
2019.435785	13446.258893	47.886861
2016.003661	13245.689442	47.891866
2012.289607	13048.737518	47.896871
2008.814550	12850.338211	47.901876
2005.458524	12646.790327	47.906881
2001.935938	12451.958024	47.911885
1998.589240	12236.477532	47.916890
1995.149200	12033.858020	47.921895
1991.643843	11848.634499	47.926900
1988.140828	11647.599255	47.931905
1984.417893	11442.193827	47.936909
1980.825730	11239.730144	47.941914
1977.971504	11037.688180	47.946919
1973.908719	10840.487867	47.951924
1970.624394	10635.757079	47.956929
1967.298939	10442.446945	47.961933
1963.954902	10234.931502	47.966938
1960.441132	10019.616577	47.971943
1956.822550	9833.224648	47.976948
1953.630402	9610.824059	47.981953
1949.736518	9409.038365	47.986957
1946.347405	9200.132889	47.991962
1942.476601	9001.785619	47.996967
1939.049971	8793.330575	48.001972
1935.840747	8595.276630	48.006977
1931.962406	8394.246552	48.011981
1928.475624	8190.109287	48.016986
1925.346039	7986.238064	48.021991
1921.407849	7782.479797	48.026996
1918.139825	7578.903773	48.032001
1914.527043	7382.888343	48.037005
1911.409108	7172.162409	48.042010
1907.984835	6962.670536	48.047015
1904.518557	6770.702571	48.052020
1900.911972	6542.899845	48.057025
1897.309323	6345.846299	48.062029
1893.809969	6129.156557	48.067034
1890.352432	5923.666316	48.072039
1886.609993	5733.705132	48.077044
1882.951311	5522.101691	48.082049
1879.659724	5313.307330	48.087053
1876.398330	5109.099427	48.092058
1872.907084	4907.208329	48.097063
1869.204886	4697.529555	48.102068
1865.904149	4491.929644	48.107073
1862.267915	4287.223164	48.112077
1858.965513	4080.862348	48.117082
1855.462743	3869.775872	48.122087
1851.482531	3661.617724	48.127092
1848.257494	3449.622465	48.132097
1844.417188	3250.756813	48.137101
1840.638430	3041.786354	48.142106
1837.173005	2839.240256	48.147111
1833.649201	2644.195362	48.152116
1830.694724	2439.855603	48.157121
1827.063684	2242.490321	48.162125
1823.429467	2034.752455	48.167130
1820.017767	1826.089891	48.172135
1815.893314	1635.067119	48.177140
1812.754565	1441.009686	48.182145
1809.128511	1239.519254	48.187149
1805.418617	1044.175995	48.192154
1801.736201	847.182159	48.197159
1797.904260	675.325832	48.202164
1794.416379	471.218547	48.207169
1790.336061	296.297823	48.212173
1786.268116	128.783369	48.217178
1780.280588	22.128982	48.222183
1769.119035	53.128248	48.227188
1762.127255	59.129554	48.232193
1757.609489	66.341405	48.237197
1754.371483	71.340802	48.242202
1752.296489	61.174427	48.247207
1750.035136	71.560795	48.252212
1747.657382	69.335486	48.257217
1744.486806	65.971898	48.262221
1741.422450	62.012712	48.267226
1738.090551	66.030210	48.272231
1734.478754	73.808980	48.277236
1731.362410	69.981320	48.282241
1728.023582	70.896217	48.287245
1724.445569	71.519512	48.292250
1720.651797	69.095033	48.297255
1716.994050	62.223113	48.302260
1714.108707	60.112054	48.307265
1710.910905	57.787302	48.312269
1707.378024	62.927772	48.317274
1703.891997	59.164308	48.322279
1700.808779	63.456112	48.327284
1697.053590	52.132170	48.332289
1693.786266	52.855550	48.337293
1690.232105	64.848978	48.342298
1686.891751	55.886749	48.347303
1682.842803	65.350647	48.352308
1679.716153	60.796946	48.357313
1676.119249	59.831824	48.362317
1672.721909	58.595022	48.367322
1669.373507	53.335703	48.372327
1666.035984	65.304724	48.377332
1662.972447	62.031980	48.382337
1659.747176	67.415392	48.387341
1655.650958	52.829181	48.392346
1651.968069	58.372800	48.397351
1648.380157	57.235436	48.402356
1645.370618	57.500864	48.407361
1641.717855	72.698848	48.412365
1638.438103	62.448975	48.417370
1635.332070	54.718776	48.422375
1631.309202	62.416373	48.427380
1627.721782	53.673173	48.432385
1624.270134	55.969356	48.437389
1620.969543	65.063043	48.442394
1617.527619	50.728796	48.447399
1614.192798	60.264444	48.452404
1610.673731	50.583562	48.457409
1607.396331	56.917955	48.462413
1603.392277	50.533728	48.467418
1600.422235	54.735075	48.472423
1596.518200	53.273880	48.477428
1592.967711	60.407167	48.482433
1589.180182	52.055977	48.487437
1586.340427	56.047109	48.492442
1583.010750	53.711402	48.497447
1579.089515	54.062596	48.502452
1575.709322	45.910256	48.507457
1572.000823	52.849975	48.512461
1568.584925	57.187555	48.517466
1565.492263	45.117732	48.522471
1561.669965	48.167981	48.527476
1558.141754	53.826625	48.532481
1554.549490	56.461218	48.537485
1550.841394	50.837459	48.542490
1547.903002	52.835031	48.547495
1544.552848	53.413232	48.552500
1540.643326	50.367858	48.557505
1537.175356	59.304261	48.562509
1533.675672	60.984725	48.567514
1530.289771	60.562440	48.572519
1526.547979	68.383760	48.577524
1523.671051	60.386784	48.582529
1520.180189	61.287577	48.587533
1516.806956	59.284581	48.592538
1513.251766	55.693369	48.597543
1509.256840	57.600055	48.602548
1505.950239	53.912987	48.607553
1501.997056	50.314472	48.612557
1498.690101	55.340546	48.617562
1495.590572	60.410086	48.622567
1492.007258	62.869291	48.627572
1488.980427	55.680413	48.632577
1484.982587	56.594134	48.637581
1481.289930	58.431371	48.642586
1478.110493	49.912283	48.647591
1474.045353	58.534046	48.652596
1470.813593	49.153109	48.657601
1467.515820	63.577379	48.662605
1464.116418	61.705049	48.667610
1460.886776	51.422102	48.672615
1457.092977	57.903805	48.677620
1453.295190	63.006723	48.682625
1449.540043	60.215634	48.687629
1445.865417	61.790631	48.692634
1443.229002	60.055146	48.697639
1439.436376	54.058682	48.702644
1436.183584	52.884758	48.707649
1432.653232	58.942414	48.712653
1428.859889	58.223268	48.717658
1425.464124	62.010405	48.722663
1422.270913	67.246492	48.727668
1419.020110	57.033311	48.732673
1415.100935	54.789938	48.737677
1411.200267	63.572642	48.742682
1407.873004	59.512352	48.747687
1404.377714	49.489314	48.752692
1401.200736	49.667128	48.757697
1397.551336	54.731016	48.762701
1393.976814	59.004892	48.767706
1390.671955	53.406665	48.772711
1386.880218	60.957430	48.777716
1383.380378	58.597809	48.782721
1379.777693	51.106804	48.787725
1376.520877	56.862227	48.792730
1373.017672	48.216691	48.797735
1369.802428	50.846112	48.802740
1365.939808	47.379014	48.807745
1362.341617	59.123145	48.812749
1359.006204	54.409245	48.817754
1355.459693	55.340953	48.822759
1351.600450	59.466422	48.827764
1348.550915	42.761318	48.832769
1345.206473	56.126717	48.837773
1341.692340	53.595341	48.842778
1338.156206	46.021172	48.847783
1334.431342	53.321034	48.852788
1331.013585	48.601055	48.857793
1327.953728	48.845980	48.862797
1323.975161	56.764535	48.867802
1320.635939	54.458889	48.872807
1316.859764	52.898696	48.877812
1313.399090	56.980768	48.882817
1309.726932	58.526953	48.887821
1306.246202	57.255876	48.892826
1303.324877	47.674550	48.897831
1299.503608	57.602803	48.902836
1296.170803	57.498157	48.907841
1292.753364	56.017858	48.912845
1289.158831	55.267645	48.917850
1285.782361	53.578453	48.922855
1281.737711	50.870720	48.927860
1278.280418	44.214387	48.932865
1275.080184	46.980694	48.937869
1271.506202	46.714493	48.942874
1268.226905	53.903496	48.947879
1264.456622	54.148923	48.952884
1260.881269	50.532492	48.957889
1257.790548	49.089646	48.962893
1254.500199	46.491634	48.967898
1250.744013	47.076549	48.972903
1246.825000	48.838572	48.977908
1243.466284	49.263189	48.982913
1239.851644	46.073701	48.987917
1236.255415	45.848961	48.992922
1233.029915	53.488300	48.997927
1229.180954	54.631917	49.002932
1225.925658	46.222884	49.007937
1222.647334	55.958593	49.012941
1219.044637	53.763834	49.017946
1215.718216	45.691810	49.022951
1211.903938	47.522873	49.027956
1208.441186	41.240751	49.032961
1205.080105	49.391707	49.037965
1201.255559	51.471156	49.042970
1197.915932	45.400718	49.047975
1194.339013	47.267395	49.052980
1191.100715	42.187180	49.057985
1187.601231	47.591499	49.062989
1183.731804	49.162285	49.067994
1180.905770	52.069356	49.072999
1177.070561	47.516033	49.078004
1173.491936	48.791357	49.083009
1169.750122	44.754931	49.088013
1166.345388	41.956558	49.093018
1163.288695	42.568038	49.098023
1159.300288	50.339488	49.103028
1155.925496	47.903429	49.108033
1152.536825	40.160722	49.113037
1149.239966	44.960685	49.118042
1145.138766	41.458267	49.123047
1141.822775	44.261719	49.128052
1138.267491	42.331656	49.133057
1135.062328	47.750025	49.138061
1131.922071	44.960878	49.143066
1128.165507	50.424448	49.148071
1124.244833	53.366869	49.153076
1120.956410	42.220070	49.158081
1117.273567	45.837108	49.163085
1113.730938	46.603777	49.168090
1110.487243	49.307336	49.173095
1106.999908	47.423594	49.178100
1103.257894	48.411309	49.183105
1099.656357	49.452964	49.188109
1096.206599	46.452856	49.193114
1093.171799	54.945070	49.198119
1089.656288	46.260455	49.203124
1086.155089	56.027929	49.208129
1082.658294	51.510248	49.213133
1078.806725	60.589093	49.218138
1075.459378	45.588560	49.223143
1072.023103	47.464898	49.228148
1068.448914	44.031863	49.233153
1064.489531	53.497752	49.238157
1060.620995	50.689775	49.243162
1058.042032	44.851477	49.248167
1054.567937	51.039645	49.253172
1051.293734	51.204321	49.258177
1047.577920	53.545217	49.263181
1043.537159	53.462916	49.268186
1040.315755	43.995116	49.273191
1036.695787	47.978828	49.278196
1033.509304	45.972079	49.283201
1029.862678	53.133238	49.288205
1026.180423	50.729547	49.293210
1023.011441	48.504925	49.298215
1019.415013	40.911861	49.303220
1016.198029	51.368849	49.308225
1012.619268	47.870112	49.313229
1008.491051	52.737012	49.318234
1005.348274	51.621942	49.323239
1001.574924	48.454236	49.328244
998.114400	51.413244	49.333249
995.119981	46.687226	49.338253
991.399923	53.138553	49.343258
987.997238	45.391779	49.348263
984.108185	52.128999	49.353268
980.498330	49.539983	49.358273
977.535394	52.550803	49.363277
974.027052	57.693986	49.368282
970.637066	38.916308	49.373287
967.071792	49.250669	49.378292
963.122093	45.069709	49.383297
959.619996	51.142068	49.388301
956.076547	52.225300	49.393306
953.030422	45.846411	49.398311
949.648970	52.039088	49.403316
946.051066	49.606404	49.408321
942.258278	57.420070	49.413325
938.373854	54.522883	49.418330
935.197055	55.646790	49.423335
931.634519	52.297406	49.428340
928.557884	50.868283	49.433345
925.245669	42.512582	49.438349
921.413893	44.302202	49.443354
917.899832	45.206839	49.448359
914.057768	46.767118	49.453364
910.665837	52.857043	49.458369
906.968335	52.195866	49.463373
903.416629	52.723586	49.468378
900.307923	38.843718	49.473383
896.803979	44.786668	49.478388
893.393294	46.798267	49.483393
889.588594	44.287256	49.488397
885.942525	40.947809	49.493402
882.767763	34.933944	49.498407
879.367883	46.368733	49.503412
875.761426	42.491573	49.508417
872.494671	41.788271	49.513421
868.625110	41.141396	49.518426
865.043313	34.805295	49.523431
861.394369	39.404212	49.528436
858.076583	49.585954	49.533441
854.972854	44.810664	49.538445
851.061521	43.202224	49.543450
848.022381	39.400757	49.548455
844.397596	47.501357	49.553460
840.616707	47.856180	49.558465
837.334271	46.971846	49.563469
833.935177	43.324826	49.568474
830.418846	36.367880	49.573479
826.823492	46.476035	49.578484
822.866249	34.978521	49.583489
819.888127	36.906589	49.588493
816.141873	35.386210	49.593498
812.793051	34.300309	49.598503
809.120517	44.335132	49.603508
805.475194	51.913777	49.608513
802.257970	42.850386	49.613517
798.831985	47.518817	49.618522
795.486106	34.679056	49.623527
791.373589	44.004496	49.628532
788.045783	44.519344	49.633537
784.836508	29.155658	49.638541
780.675731	44.907945	49.643546
777.762209	36.531005	49.648551
774.510017	35.512244	49.653556
770.593222	46.059896	49.658561
767.254391	43.732248	49.663565
763.402235	48.499066	49.668570
760.322602	31.821106	49.673575
756.594919	41.636788	49.678580
753.003306	43.923543	49.683585
750.071456	38.400038	49.688589
745.946402	42.001038	49.693594
742.734569	39.786391	49.698599
739.146156	36.605658	49.703604
735.254159	39.588031	49.708609
732.297908	41.468408	49.713613
728.465299	53.432917	49.718618
725.004671	40.930695	49.723623
721.573622	35.820738	49.728628
717.791675	36.954062	49.733633
714.747550	29.578370	49.738637
710.866587	41.550450	49.743642
707.833162	32.765207	49.748647
703.872595	39.766823	49.753652
700.406671	39.793966	49.758657
697.453682	33.827702	49.763661
693.821409	34.459867	49.768666
690.095492	37.011287	49.773671
686.382115	39.987853	49.778676
683.046238	42.117523	49.783681
679.891646	34.718014	49.788685
676.034490	33.325793	49.793690
672.627768	30.483632	49.798695
669.044512	38.878338	49.803700
665.379281	48.658963	49.808705
662.228486	38.098261	49.813709
658.478421	39.204470	49.818714
655.298555	28.980525	49.823719
651.446267	34.073270	49.828724
648.053206	38.284174	49.833729
644.573454	36.336150	49.838733
640.730725	44.002709	49.843738
637.857835	31.554023	49.848743
634.193097	43.868753	49.853748
630.360762	36.094514	49.858753
626.731835	37.877792	49.863757
623.170772	36.429731	49.868762
620.231658	31.669881	49.873767
616.268633	40.655595	49.878772
613.180248	34.479612	49.883777
610.056175	35.101822	49.888781
605.830915	41.705167	49.893786
602.772484	35.249249	49.898791
599.039085	39.016761	49.903796
595.476355	33.310546	49.908801
592.059938	33.092694	49.913805
588.193870	40.718634	49.918810
584.988797	35.060812	49.923815
581.234382	41.362633	49.928820
577.690458	43.157927	49.933825
574.115951	38.364729	49.938829
570.703436	49.130863	49.943834
567.645345	40.080617	49.948839
564.089364	42.637108	49.953844
560.760589	41.791771	49.958849
557.420717	40.913372	49.963853
553.187138	46.869471	49.968858
549.590058	43.652208	49.973863
546.708054	43.078589	49.978868
543.052664	47.175592	49.983873
539.484922	46.437292	49.988877
535.959076	49.023876	49.993882
532.348075	35.618321	49.998887
528.869906	44.695807	50.003892
525.190668	40.453709	50.008897
521.954040	35.749984	50.013901
518.299940	43.342750	50.018906
515.150811	41.472708	50.023911
511.211788	39.976322	50.028916
507.820859	45.616961	50.033921
504.481141	42.584035	50.038925
500.542654	44.738551	50.043930
497.777112	38.157705	50.048935
493.927651	42.262976	50.053940
490.350832	33.123170	50.058945
486.886354	34.558041	50.063949
483.181293	36.944922	50.068954
480.041178	31.704077	50.073959
476.601670	39.389795	50.078964
472.865772	39.642808	50.083969
469.304812	42.067236	50.088973
465.157546	42.163222	50.093978
462.288146	28.739628	50.098983
458.948780	36.219839	50.103988
455.182257	41.716843	50.108993
452.073070	34.775389	50.113997
448.373557	40.910470	50.119002
445.214043	39.734944	50.124007
441.147522	47.452448	50.129012
437.968775	39.465196	50.134017
434.437121	32.422244	50.139021
430.455814	35.023258	50.144026
427.038996	31.271613	50.149031
423.592786	36.193272	50.154036
420.746430	39.515025	50.159041
417.206778	29.341212	50.164045
413.185193	39.364392	50.169050
409.703913	37.644493	50.174055
406.366538	38.214761	50.179060
402.615032	41.032893	50.184065
399.096779	39.375737	50.189069
395.764773	36.009453	50.194074
392.401930	39.060939	50.199079
388.738735	33.196546	50.204084
385.282021	32.364989	50.209089
381.917790	29.968706	50.214093
378.128705	35.276282	50.219098
375.074241	45.385270	50.224103
371.800893	36.903501	50.229108
367.853838	39.654201	50.234113
364.491679	29.639274	50.239117
360.296973	42.590757	50.244122
357.172765	36.100947	50.249127
353.819435	37.765231	50.254132
350.171802	41.927528	50.259137
346.583889	39.221446	50.264141
342.561104	31.382271	50.269146
339.818797	30.448316	50.274151
336.307001	40.888378	50.279156
332.756864	36.736876	50.284161
329.737218	36.134268	50.289165
325.593362	34.916827	50.294170
322.349670	34.441067	50.299175
318.512781	34.909281	50.304180
314.988011	39.672441	50.309185
311.806847	42.356974	50.314189
308.169537	38.605116	50.319194
304.847042	25.983398	50.324199
301.339156	26.434883	50.329204
297.846942	38.143717	50.334209
294.342146	31.381359	50.339213
290.603413	40.214997	50.344218
286.880722	35.555871	50.349223
283.549978	39.519855	50.354228
280.374681	40.295735	50.359233
276.630471	35.310954	50.364237
272.674498	47.108269	50.369242
270.015874	38.001900	50.374247
266.171888	34.785474	50.379252
262.535866	28.239842	50.384257
259.114729	30.449456	50.389261
255.304873	40.262356	50.394266
252.147831	42.772288	50.399271
248.832782	41.630690	50.404276
245.225698	35.979036	50.409281
241.801511	38.894652	50.414285
238.199959	40.240359	50.419290
234.355002	40.874389	50.424295
230.702075	36.951005	50.429300
227.447220	37.103453	50.434305
224.230334	33.690731	50.439309
220.905477	46.474361	50.444314
217.371840	42.712629	50.449319
213.523876	50.187176	50.454324
210.000186	42.668512	50.459329
206.845120	45.491361	50.464333
202.965340	48.190464	50.469338
199.504811	37.162799	50.474343
196.333168	34.461173	50.479348
192.597794	34.353554	50.484353
189.082580	34.230429	50.489357
185.170160	40.319866	50.494362
182.037993	33.530820	50.499367
179.005857	46.097760	50.504372
174.831844	46.470155	50.509377
171.604350	40.515457	50.514381
168.036982	46.639431	50.519386
164.793267	45.056420	50.524391
161.281630	49.295561	50.529396
157.426623	39.649002	50.534401
153.633419	39.882654	50.539405
150.241125	43.992369	50.544410
146.955281	44.956458	50.549415
143.823128	34.234882	50.554420
140.129568	40.843706	50.559425
136.767786	44.632271	50.564429
132.935572	43.536940	50.569434
129.560628	38.750639	50.574439
126.110039	37.057685	50.579444
122.267240	45.126241	50.584449
118.871027	33.101452	50.589453
115.266097	37.216019	50.594458
111.960714	38.588142	50.599463
108.760298	38.877637	50.604468
105.179934	42.456850	50.609473
101.885019	30.526932	50.614477
98.150924	33.665160	50.619482
94.719725	36.534472	50.624487
91.082303	39.894839	50.629492
87.201190	41.559653	50.634497
84.060096	34.598040	50.639501
80.110136	32.818829	50.644506
76.814838	40.513720	50.649511
73.455053	35.449823	50.654516
69.724414	40.064993	50.659521
66.536324	39.390793	50.664525
63.216660	42.505234	50.669530
59.472996	35.859502	50.674535
56.074511	34.670941	50.679540
52.315752	37.069571	50.684545
49.086326	39.733282	50.689549
45.342446	43.069218	50.694554
42.066967	39.953649	50.699559
38.443817	40.113251	50.704564
34.600653	38.703306	50.709569
31.273530	34.703657	50.714573
27.784696	39.768175	50.719578
24.572868	36.981162	50.724583
21.156132	46.754699	50.729588
17.343722	47.507111	50.734593
14.152418	40.436334	50.739597
10.063195	42.244519	50.744602
6.668334	40.058830	50.749607
3.911122	41.205899	50.754612