Thu Aug 25 10:28:34 2022

Number of Points = 9925

Depth (nm)	Load (N)	Time (s)
2.597720	96.378508	0.000000
1.940134	85.572953	0.005005
1.930283	90.313834	0.010010
2.185169	94.953126	0.015014
1.937598	89.230756	0.020019
1.221807	72.135297	0.025024
1.242193	75.504696	0.030029
1.186920	70.226765	0.035034
1.174720	72.168092	0.040038
0.831676	63.379196	0.045043
0.838133	56.060471	0.050048
0.097475	45.021184	0.055053
0.000671	47.640150	0.060058
-0.105884	27.788567	0.065062
-0.761363	32.918492	0.070067
-0.711188	17.610810	0.075072
-1.404100	22.234071	0.080077
-2.246023	19.085222	0.085082
-1.767378	13.261746	0.090086
-1.874844	12.152328	0.095091
-1.989688	0.742934	0.100096
-2.563995	4.148551	0.105101
-2.628781	-4.800967	0.110106
-3.096943	-3.180511	0.115110
-3.672859	5.806191	0.120115
-3.626641	-5.014670	0.125120
-3.551063	4.891841	0.130125
-4.506918	6.278665	0.135130
-5.082406	-2.714222	0.140134
-5.630900	-2.732650	0.145139
-5.564490	-2.116599	0.150144
-5.844165	2.641225	0.155149
-5.565575	-7.172009	0.160154
-5.761313	-6.685726	0.165158
-5.979197	0.191611	0.170163
-5.620043	-15.499810	0.175168
-5.997374	0.839933	0.180173
-6.903442	-5.886539	0.185178
-6.888158	-3.661627	0.190182
-7.339198	0.139125	0.195187
-7.238056	-3.825031	0.200192
-8.294591	-4.042266	0.205197
-8.502694	-1.519763	0.210202
-8.703183	-8.869311	0.215206
-8.820513	-8.018829	0.220211
-8.528998	-3.002491	0.225216
-8.463108	-2.206026	0.230221
-9.108973	-2.326256	0.235226
-9.732153	-1.561030	0.240230
-10.317962	-4.655090	0.245235
-10.032881	-9.046695	0.250240
-10.279252	-4.287763	0.255245
-10.203656	3.862870	0.260250
-10.692548	-2.698014	0.265254
-11.291199	4.052324	0.270259
-11.201427	0.555019	0.275264
-11.470354	7.386572	0.280269
-11.888432	3.744213	0.285274
-12.808519	-4.008277	0.290278
-12.544383	6.928542	0.295283
-12.510182	-2.558502	0.300288
-12.934819	-6.354855	0.305293
-13.049244	-5.096706	0.310298
-12.966033	-12.819732	0.315302
-13.218875	-5.604728	0.320307
-13.884827	-8.132577	0.325312
-14.246297	0.928090	0.330317
-14.485317	-1.723600	0.335322
-14.527503	-2.760988	0.340326
-14.929760	-4.842938	0.345331
-14.686398	2.455672	0.350336
-15.974259	7.811225	0.355341
-16.058533	1.231235	0.360346
-15.787290	-3.338536	0.365350
-16.219833	0.127125	0.370355
-16.138318	-5.491752	0.375360
-16.308607	3.858498	0.380365
-16.470405	-10.836981	0.385370
-17.014844	-4.126778	0.390374
-17.626849	4.745356	0.395379
-17.665978	-1.762612	0.400384
-17.769533	5.811818	0.405389
-18.147936	5.712956	0.410394
-18.460454	1.892707	0.415398
-19.134626	-6.426655	0.420403
-19.000042	1.509091	0.425408
-19.296251	2.545788	0.430413
-19.107323	-4.633824	0.435418
-18.726576	-10.242638	0.440422
-19.886941	2.261962	0.445427
-20.266264	-2.626653	0.450432
-20.399511	-0.546147	0.455437
-20.463796	1.077467	0.460442
-20.421509	-10.666584	0.465446
-21.107480	4.626868	0.470451
-20.985220	-0.691513	0.475456
-21.470763	0.023675	0.480461
-21.446884	-2.526839	0.485466
-21.763019	3.252258	0.490470
-22.304945	2.824680	0.495475
-22.636243	-10.312991	0.500480
-23.138703	6.900570	0.505485
-23.785241	-1.840738	0.510490
-23.564549	-2.966770	0.515494
-24.085547	4.862890	0.520499
-23.973313	2.893314	0.525504
-24.508439	6.008057	0.530509
-24.324149	-4.752179	0.535514
-24.433637	1.845584	0.540518
-24.559252	9.651261	0.545523
-24.633759	3.243747	0.550528
-25.197535	5.850453	0.555533
-25.754394	2.549377	0.560538
-25.691065	0.963949	0.565542
-25.960646	-0.275089	0.570547
-26.514500	8.831543	0.575552
-27.106601	14.571626	0.580557
-27.191312	5.663192	0.585562
-27.497540	1.281977	0.590566
-27.603360	11.897115	0.595571
-27.746468	4.804326	0.600576
-27.941548	12.798058	0.605581
-27.726305	-0.991564	0.610586
-27.711404	4.776794	0.615590
-28.687929	7.277330	0.620595
-28.743119	-3.502330	0.625600
-28.998188	-1.640017	0.630605
-29.546510	2.201289	0.635610
-30.136039	7.311383	0.640614
-30.025799	8.679863	0.645619
-30.122099	0.684404	0.650624
-30.173856	11.088592	0.655629
-30.515192	7.991026	0.660634
-30.463982	6.872566	0.665638
-31.370502	11.133828	0.670643
-31.074437	-0.513951	0.675648
-31.842704	6.658431	0.680653
-31.775086	5.910721	0.685658
-31.890365	1.404675	0.690662
-32.763328	7.723435	0.695667
-32.951683	3.776165	0.700672
-33.212553	4.832635	0.705677
-33.146512	-0.682579	0.710682
-33.169359	1.788751	0.715686
-33.599101	0.372329	0.720691
-33.483562	3.771097	0.725696
-34.320123	6.028242	0.730701
-34.556080	8.861993	0.735706
-34.809843	3.415869	0.740710
-34.947445	9.945273	0.745715
-35.076181	0.240151	0.750720
-35.040664	4.385445	0.755725
-36.077356	-5.019223	0.760730
-36.406222	-8.200996	0.765734
-36.882020	-4.845616	0.770739
-36.753760	-2.913652	0.775744
-36.712365	7.033014	0.780749
-36.783642	1.453894	0.785754
-36.291149	-3.761144	0.790758
-36.894331	-2.562454	0.795763
-37.268759	-7.325284	0.800768
-38.160218	0.065714	0.805773
-38.433266	1.513232	0.810778
-38.112151	-3.092827	0.815782
-39.024161	-2.124157	0.820787
-39.102835	-9.391549	0.825792
-39.444144	-2.235449	0.830797
-39.694702	-1.231214	0.835802
-39.591314	-8.008281	0.840806
-40.043665	-3.571413	0.845811
-39.510791	-8.207487	0.850816
-40.086770	5.831710	0.855821
-41.027511	4.761109	0.860826
-40.902095	-1.861225	0.865830
-41.191742	-5.960299	0.870835
-41.011242	-8.744159	0.875840
-42.115452	-4.550000	0.880845
-42.312243	4.753781	0.885850
-42.407666	1.013413	0.890854
-42.481511	2.610051	0.895859
-42.324584	-4.520253	0.900864
-42.442527	-0.474301	0.905869
-42.741928	-1.866853	0.910874
-43.304095	-5.046872	0.915878
-43.725539	-2.566871	0.920883
-43.746529	3.365296	0.925888
-44.100480	10.773317	0.930893
-45.045573	5.815164	0.935898
-45.309889	7.052508	0.940902
-45.497412	7.034470	0.945907
-44.733578	-0.640181	0.950912
-45.214750	11.043000	0.955917
-45.556143	6.613511	0.960922
-45.437931	4.544923	0.965926
-46.225161	10.258632	0.970931
-46.534363	-2.135862	0.975936
-46.716732	3.062294	0.980941
-46.885457	9.017611	0.985946
-46.541460	-5.839377	0.990950
-47.811999	9.295737	0.995955
-48.068471	0.097846	1.000960
-48.440076	-1.058767	1.005965
-48.626144	2.656177	1.010970
-48.630633	8.022614	1.015974
-48.669530	5.988134	1.020979
-48.418341	10.071161	1.025984
-48.695459	4.166792	1.030989
-49.453233	2.912500	1.035994
-49.559752	-1.537970	1.040998
-49.964284	3.970241	1.046003
-50.064273	8.190551	1.051008
-50.787955	4.703646	1.056013
-51.268183	6.822702	1.061018
-51.401708	3.186379	1.066022
-51.332613	14.349910	1.071027
-51.105077	8.141841	1.076032
-51.178538	9.833332	1.081037
-51.775996	11.559471	1.086042
-51.721355	1.107448	1.091046
-52.766675	10.958636	1.096051
-53.042023	5.594988	1.101056
-52.886902	6.877342	1.106061
-53.325539	6.427254	1.111066
-53.117783	4.449039	1.116070
-53.807469	10.919416	1.121075
-53.957887	9.497193	1.126080
-54.391811	10.115709	1.131085
-54.323278	8.273203	1.136090
-54.189390	-5.035433	1.141094
-54.744483	3.929023	1.146099
-55.414258	1.844699	1.151104
-55.518468	-2.077788	1.156109
-55.959374	4.163782	1.161114
-55.613691	6.669116	1.166118
-55.850340	8.370358	1.171123
-56.247157	2.434125	1.176128
-56.900938	-1.762916	1.181133
-57.003833	3.568319	1.186138
-56.754394	-1.608637	1.191142
-57.549804	4.609386	1.196147
-58.087555	8.667335	1.201152
-58.258788	8.203822	1.206157
-58.616575	8.993906	1.211162
-58.502227	10.247847	1.216166
-58.944481	20.589839	1.221171
-58.753653	3.004392	1.226176
-58.847450	13.048172	1.231181
-59.570088	17.173057	1.236186
-59.649719	10.016539	1.241190
-59.997055	11.102377	1.246195
-60.296574	2.082074	1.251200
-60.463987	1.048490	1.256205
-60.521870	1.560629	1.261210
-60.855300	1.812225	1.266214
-62.071042	3.344179	1.271219
-61.692276	-0.078185	1.276224
-61.904107	0.277743	1.281229
-61.854752	-1.428881	1.286234
-61.840552	-1.114696	1.291238
-62.108591	9.329704	1.296243
-62.915688	7.282716	1.301248
-63.481384	8.817218	1.306253
-63.567841	5.790449	1.311258
-63.539141	6.754092	1.316262
-63.687294	12.269590	1.321267
-63.887159	-0.812747	1.326272
-63.786385	-0.034404	1.331277
-64.462779	9.686212	1.336282
-64.817002	6.796311	1.341286
-65.214413	5.937970	1.346291
-65.296684	-2.246344	1.351296
-65.340700	-1.635138	1.356301
-65.628462	2.238108	1.361306
-66.249731	2.120356	1.366310
-66.517189	10.021022	1.371315
-66.624998	3.675675	1.376320
-66.692292	6.745588	1.381325
-66.596535	11.242110	1.386330
-66.730210	2.683036	1.391334
-68.054651	8.582161	1.396339
-67.977333	-9.235422	1.401344
-67.933558	3.748051	1.406349
-68.165408	7.976366	1.411354
-67.698577	-0.129472	1.416358
-68.626985	8.336662	1.421363
-68.999412	4.408746	1.426368
-69.054482	1.655468	1.431373
-69.190511	1.233896	1.436378
-69.628272	-1.854884	1.441382
-70.607865	5.818845	1.446387
-70.602884	0.702339	1.451392
-70.626435	2.771984	1.456397
-70.481652	-0.667501	1.461402
-70.376982	2.267900	1.466406
-70.792867	1.991417	1.471411
-71.439168	-5.291436	1.476416
-71.799317	-3.903036	1.481421
-72.087904	3.459939	1.486426
-72.010318	-8.368733	1.491430
-72.905966	7.723196	1.496435
-73.380930	1.565094	1.501440
-73.529663	-9.832648	1.506445
-73.304455	4.296142	1.511450
-73.573631	1.203092	1.516454
-73.619021	0.821101	1.521459
-73.854596	-0.435919	1.526464
-73.942121	3.820401	1.531469
-74.096179	-1.423044	1.536474
-74.520244	2.582290	1.541478
-75.268978	2.611061	1.546483
-75.304622	7.998197	1.551488
-75.638594	1.678798	1.556493
-75.872376	4.331875	1.561498
-76.459663	-7.171156	1.566502
-76.790482	-10.801870	1.571507
-76.907766	-9.315484	1.576512
-77.006647	1.921812	1.581517
-76.850204	10.474225	1.586522
-76.837829	4.910472	1.591526
-76.824297	6.771828	1.596531
-77.119512	-0.850775	1.601536
-78.229748	-0.240179	1.606541
-78.574059	7.172657	1.611546
-78.201425	6.851714	1.616550
-78.492525	16.477160	1.621555
-79.048857	-4.904747	1.626560
-79.361083	-3.115735	1.631565
-79.757256	-4.353917	1.636570
-79.701983	0.291312	1.641574
-79.981780	5.188361	1.646579
-80.198877	2.093479	1.651584
-81.025072	0.403824	1.656589
-81.229007	9.411334	1.661594
-81.241865	2.190575	1.666598
-81.384416	8.622677	1.671603
-81.951523	-5.212027	1.676608
-81.310162	3.267563	1.681613
-81.383443	-1.586744	1.686618
-81.831594	-3.212249	1.691622
-82.434058	6.579037	1.696627
-82.837634	-4.671208	1.701632
-83.116843	5.907817	1.706637
-83.208224	1.723893	1.711642
-83.696532	2.721090	1.716646
-84.247921	8.730038	1.721651
-84.275566	1.116129	1.726656
-84.295518	-3.901556	1.731661
-84.358679	8.146390	1.736666
-84.339116	-5.479684	1.741670
-84.948568	8.026922	1.746675
-85.750688	3.498788	1.751680
-85.732716	3.758598	1.756685
-85.936161	7.514229	1.761690
-85.821423	3.032255	1.766694
-86.109818	7.269430	1.771699
-86.193583	2.733139	1.776704
-86.637224	-2.003024	1.781709
-87.240626	-1.329477	1.786714
-87.388586	2.123232	1.791718
-87.531313	3.243448	1.796723
-87.466967	-6.090125	1.801728
-88.018188	-1.359355	1.806733
-88.517952	5.986090	1.811738
-88.764787	-0.647515	1.816742
-88.889870	4.035466	1.821747
-88.927315	-6.664709	1.826752
-88.740007	5.315515	1.831757
-89.461714	6.412558	1.836762
-89.556133	-4.424223	1.841766
-90.638467	5.167010	1.846771
-90.237382	4.620147	1.851776
-89.936481	-3.181281	1.856781
-90.778450	-2.884801	1.861786
-91.254271	-9.485686	1.866790
-91.448875	1.965923	1.871795
-91.404602	-11.423574	1.876800
-92.017212	2.023412	1.881805
-92.174008	-0.068523	1.886810
-92.526311	-5.837718	1.891814
-92.996340	6.058845	1.896819
-93.454600	1.802697	1.901824
-92.844357	-0.333498	1.906829
-93.182138	-0.150821	1.911834
-92.971048	-5.457807	1.916838
-93.400804	0.168250	1.921843
-93.641968	1.575972	1.926848
-94.435234	-0.466851	1.931853
-95.300824	3.446316	1.936858
-94.609781	0.120551	1.941862
-94.943638	-2.829484	1.946867
-95.128055	-5.429614	1.951872
-95.528499	-9.299353	1.956877
-95.919117	2.391777	1.961882
-95.929077	0.722922	1.966886
-96.323844	8.621388	1.971891
-96.400141	0.714549	1.976896
-96.789124	2.825636	1.981901
-97.490753	1.499276	1.986906
-97.594150	3.916789	1.991910
-97.921370	4.505933	1.996915
-97.954858	0.657992	2.006912
-97.810261	0.834977	2.016909
-96.785314	12.445942	2.026906
-96.677524	4.373441	2.036902
-96.010046	7.094588	2.046899
-95.409520	2.923620	2.056896
-95.198360	10.781562	2.066893
-94.653293	14.662295	2.076890
-93.732018	11.299537	2.086886
-93.650115	3.997696	2.096883
-93.274937	9.476272	2.106880
-92.750700	11.199838	2.116877
-92.364679	12.783504	2.126874
-91.124015	0.542079	2.136870
-91.234802	6.353391	2.146867
-90.937583	7.878113	2.156864
-90.111483	10.694783	2.166861
-89.498425	6.249421	2.176858
-88.553797	2.201931	2.186854
-88.029390	8.220989	2.196851
-88.249094	2.325389	2.206848
-87.938106	3.432973	2.216845
-87.548384	6.850208	2.226842
-86.734331	4.213837	2.236838
-85.714687	6.509173	2.246835
-85.554083	-5.052998	2.256832
-85.248195	2.726742	2.266829
-84.337992	4.560891	2.276826
-83.864226	1.398135	2.286822
-83.780484	-0.464903	2.296819
-82.942361	0.658285	2.306816
-82.618003	2.368822	2.316813
-82.368456	3.460691	2.326810
-81.417396	0.872544	2.336806
-81.204647	0.227896	2.346803
-80.641222	0.801751	2.356800
-79.761289	5.349101	2.366797
-79.574944	7.040083	2.376794
-79.052949	4.965824	2.386790
-78.671169	8.656734	2.396787
-78.311465	0.776009	2.406784
-76.987586	3.932830	2.416781
-77.159959	5.372743	2.426778
-76.910403	7.424451	2.436774
-75.699643	7.180955	2.446771
-75.315818	3.582466	2.456768
-75.198333	1.539913	2.466765
-74.735928	9.358488	2.476762
-73.850331	8.206103	2.486758
-73.636188	5.324779	2.496755
-72.508617	6.994991	2.506752
-72.448437	0.181226	2.516749
-72.478701	2.679087	2.526746
-71.629319	5.067627	2.536742
-71.082943	-3.073594	2.546739
-70.344709	-0.005572	2.556736
-69.769693	-0.152620	2.566733
-69.865567	5.710209	2.576730
-69.282575	3.974849	2.586726
-68.730410	1.309823	2.596723
-67.798702	-0.271102	2.606720
-67.028812	1.778269	2.616717
-67.002884	-1.795817	2.626714
-67.059032	8.419662	2.636710
-65.932514	3.592907	2.646707
-65.458957	0.297138	2.656704
-65.210571	8.580067	2.666701
-65.028304	10.417407	2.676698
-63.742054	7.136846	2.686694
-63.117423	2.436249	2.696691
-62.983878	2.263342	2.706688
-62.739242	0.796409	2.716685
-61.687708	7.733896	2.726682
-61.637509	3.525615	2.736678
-61.356368	4.181716	2.746675
-60.407183	1.479824	2.756672
-59.784591	-2.979700	2.766669
-59.440294	5.661999	2.776666
-58.717974	8.602639	2.786662
-58.483093	5.436132	2.796659
-58.436970	4.988654	2.806656
-57.701246	2.348719	2.816653
-57.162426	0.183128	2.826650
-56.219503	-2.172494	2.836646
-55.637102	3.789963	2.846643
-55.660700	-0.083639	2.856640
-54.912240	5.266758	2.866637
-54.350587	4.393213	2.876634
-53.927860	2.816014	2.886630
-53.285045	4.147203	2.896627
-52.793414	7.317225	2.906624
-52.641697	8.649337	2.916621
-52.194581	4.819186	2.926618
-51.684936	-0.918266	2.936614
-51.046245	1.601490	2.946611
-50.214620	-4.785123	2.956608
-49.853264	-4.718128	2.966605
-49.766682	-4.085394	2.976602
-48.902239	-5.034891	2.986598
-48.228855	0.678893	2.996595
-48.035062	-2.389308	3.006592
-47.524164	-4.284430	3.016589
-46.927116	-7.200406	3.026586
-46.612089	-4.709131	3.036582
-45.824459	-5.706780	3.046579
-45.368887	-9.161286	3.056576
-45.083662	-3.120589	3.066573
-44.313922	1.234957	3.076570
-44.034438	0.003317	3.086566
-43.564734	-1.479874	3.096563
-42.695957	-2.468063	3.106560
-42.396013	-9.455609	3.116557
-42.238550	-3.949255	3.126554
-41.163390	-0.091390	3.136550
-40.929413	3.309070	3.146547
-40.749700	1.833303	3.156544
-40.102546	-11.214769	3.166541
-39.419121	-9.440117	3.176538
-38.174554	-7.902273	3.186534
-38.747108	-7.723792	3.196531
-37.744952	-7.560799	3.206528
-37.650765	-6.371727	3.216525
-36.945477	-4.359747	3.226522
-36.572649	-0.708614	3.236518
-36.077030	0.680486	3.246515
-35.282930	-1.487090	3.256512
-35.104073	-0.061029	3.266509
-33.976068	5.914144	3.276506
-33.577435	3.415726	3.286502
-33.877415	5.734105	3.296499
-33.285576	0.566647	3.306496
-32.278012	-0.167690	3.316493
-32.103171	-4.424010	3.326490
-30.938567	-1.080668	3.336486
-30.586937	2.326700	3.346483
-30.464320	-1.455773	3.356480
-30.385223	2.051317	3.366477
-29.260694	-0.402448	3.376474
-29.039708	-1.754802	3.386470
-28.486777	4.462531	3.396467
-27.822086	7.554754	3.406464
-27.537442	4.092182	3.416461
-26.677410	0.910087	3.426458
-26.318626	6.318377	3.436454
-26.208120	3.180862	3.446451
-25.314256	6.310036	3.456448
-24.856228	2.329291	3.466445
-24.374292	-5.085914	3.476442
-24.016606	1.453447	3.486438
-23.631272	-3.992096	3.496435
-23.032957	-8.970499	3.506432
-22.476863	-4.540295	3.516429
-21.747544	-2.668294	3.526426
-20.978245	0.933390	3.536422
-20.842669	1.476085	3.546419
-20.781759	-0.228153	3.556416
-19.702654	-0.267282	3.566413
-19.036859	1.107827	3.576410
-19.111454	-7.446111	3.586406
-18.805249	-5.336754	3.596403
-17.844714	-5.338297	3.606400
-17.453422	-2.523184	3.616397
-16.520918	-2.194053	3.626394
-16.444958	3.524645	3.636390
-16.088816	1.821665	3.646387
-14.849990	3.997138	3.656384
-14.650667	7.624775	3.666381
-14.653904	7.292736	3.676378
-14.175781	11.412047	3.686374
-13.209641	7.966238	3.696371
-12.940209	9.241895	3.706368
-12.108405	4.971335	3.716365
-11.653862	2.448319	3.726362
-11.579087	6.681512	3.736358
-11.138198	7.882786	3.746355
-10.483609	6.430816	3.756352
-9.730988	5.958172	3.766349
-9.186402	5.606822	3.776346
-8.687026	0.697772	3.786342
-8.745062	4.901089	3.796339
-7.562775	5.970360	3.806336
-7.010239	4.312635	3.816333
-7.312781	4.166875	3.826330
-6.461132	4.638555	3.836326
-5.603017	6.550566	3.846323
-5.381929	5.692372	3.856320
-5.026021	13.286891	3.866317
-4.496192	14.604111	3.876314
-3.740770	32.805165	3.886310
-3.422077	28.643507	3.896307
-3.193701	35.082767	3.906304
-2.751480	33.445492	3.916301
-2.411632	54.302937	3.926298
-1.896040	59.449092	3.936294
-1.546372	73.535437	3.946291
-0.972019	95.819713	3.956288
-0.224419	112.111888	3.966285
0.000000	114.840978	3.971290
0.376212	114.737776	3.976294
0.590466	128.254622	3.981299
0.771786	138.043399	3.986304
0.695626	144.772035	3.991309
0.707448	141.929160	3.996314
0.597437	137.124859	4.001318
0.426243	132.624375	4.006323
0.472666	125.894146	4.011328
1.098923	147.363422	4.016333
0.778713	150.726090	4.021338
1.196142	151.923064	4.026342
1.362542	159.002845	4.031347
1.463302	140.178516	4.036352
1.130096	139.123442	4.041357
0.756491	142.630516	4.046362
0.910840	138.477658	4.051366
0.769109	145.289335	4.056371
1.168845	151.250546	4.061376
0.953207	147.408757	4.066381
1.088751	157.524258	4.071386
1.424659	152.159701	4.076390
1.084047	149.640964	4.081395
0.855459	140.435463	4.086400
0.889948	149.434165	4.091405
1.193136	160.684502	4.096410
1.225335	149.637953	4.101414
1.234544	160.586336	4.106419
1.217690	155.988897	4.111424
1.588746	154.639979	4.116429
1.357402	149.231424	4.121434
1.420174	134.427870	4.126438
1.225192	146.879387	4.131443
1.233544	138.984526	4.136448
0.915213	135.804238	4.141453
1.383411	157.098974	4.146458
1.778435	139.936973	4.151462
1.182802	143.785720	4.156467
1.085637	149.052827	4.161472
1.343093	146.193611	4.166477
1.120897	151.613187	4.171482
1.757591	148.786299	4.176486
1.303203	168.238758	4.181491
1.495338	152.329748	4.186496
1.349691	148.556087	4.191501
1.238000	163.174399	4.196506
1.742535	154.198874	4.201510
1.650707	152.644070	4.206515
1.441925	140.230573	4.211520
1.194640	140.576239	4.216525
1.167280	151.425942	4.221530
1.351555	141.598930	4.226534
1.575180	148.796290	4.231539
1.520570	152.256549	4.236544
1.722733	156.337804	4.241549
1.587413	152.040503	4.246554
1.637067	153.624133	4.251558
1.350727	159.699169	4.256563
1.277232	148.890645	4.261568
1.446508	156.855827	4.266573
1.591587	160.965010	4.271578
1.559175	145.939078	4.276582
1.568730	155.767432	4.281587
1.379281	156.724134	4.286592
1.469495	161.348116	4.291597
1.409327	156.434759	4.296602
1.513164	153.299053	4.301606
1.565876	161.187588	4.306611
1.528061	153.113292	4.311616
1.738442	165.599386	4.316621
1.771147	170.887281	4.321626
1.859991	158.120253	4.326630
1.910506	158.624904	4.331635
1.592200	159.032318	4.336640
1.700343	154.567155	4.341645
1.506091	152.708859	4.346650
1.855661	160.924206	4.351654
1.428600	158.485452	4.356659
1.854383	174.886183	4.361664
2.085873	178.776186	4.366669
1.865027	178.709584	4.371674
1.875137	178.863060	4.376678
2.100502	179.583926	4.381683
2.055992	169.694668	4.386688
1.801797	162.660348	4.391693
1.865812	165.716044	4.396698
1.778865	162.110354	4.401702
1.846019	176.662690	4.406707
2.224577	166.735620	4.411712
2.054207	169.150994	4.416717
1.541772	162.286851	4.421722
2.067546	173.151142	4.426726
1.673382	174.731545	4.431731
2.046967	184.385819	4.436736
2.429007	186.341318	4.441741
2.090099	182.338501	4.446746
2.101665	178.078290	4.451750
2.270630	180.244344	4.456755
1.831219	174.450764	4.461760
1.899033	187.253441	4.466765
2.048087	186.410707	4.471770
2.095242	182.714398	4.476774
2.286104	194.621437	4.481779
2.503279	190.094890	4.486784
2.255077	182.850814	4.491789
2.114614	177.061013	4.496794
2.167951	159.500111	4.501798
1.718626	166.682694	4.506803
2.345979	176.974250	4.511808
2.103211	183.918832	4.516813
2.282007	192.331794	4.521818
2.066590	183.763289	4.526822
2.295014	195.284791	4.531827
2.013353	193.712270	4.536832
2.281800	180.439356	4.541837
1.805201	191.628392	4.546842
2.289610	186.503151	4.551846
2.048594	188.230403	4.556851
2.227442	185.190507	4.561856
2.220816	186.264099	4.566861
2.102908	181.407239	4.571866
2.337863	178.152908	4.576870
2.215922	189.713483	4.581875
2.403243	187.074058	4.586880
1.950969	180.023311	4.591885
2.793467	202.885634	4.596890
2.778765	198.053728	4.601894
2.545870	195.742735	4.606899
2.470050	191.296895	4.611904
2.359823	187.780269	4.616909
2.387440	186.754080	4.621914
2.448056	183.973155	4.626918
2.232618	191.293111	4.631923
2.337407	190.109296	4.636928
2.822433	201.312185	4.641933
2.754182	205.926205	4.646938
2.845187	199.119361	4.651942
2.668807	183.571785	4.656947
2.691534	185.472850	4.661952
2.592574	185.333366	4.666957
2.582955	191.751036	4.671962
2.593872	187.076472	4.676966
2.542688	188.609464	4.681971
2.412253	194.242468	4.686976
2.493840	187.639584	4.691981
2.696570	204.078455	4.696986
3.112339	198.540019	4.701990
2.626016	200.906824	4.706995
2.550252	192.708742	4.712000
2.647577	193.389558	4.717005
2.608977	198.236213	4.722010
2.696665	198.061158	4.727014
2.631207	189.380568	4.732019
2.929026	211.803058	4.737024
2.910959	204.064168	4.742029
2.754559	201.238149	4.747034
2.877239	201.320204	4.752038
2.539249	195.051979	4.757043
2.909946	212.840780	4.762048
2.885230	208.551446	4.767053
2.702287	225.617080	4.772058
3.006984	214.796716	4.777062
2.987211	213.252763	4.782067
3.139114	210.141154	4.787072
2.985766	197.782206	4.792077
2.736316	197.103150	4.797082
3.009291	199.401607	4.802086
2.859281	206.065908	4.807091
3.048670	203.574853	4.812096
2.920187	202.519337	4.817101
2.946818	207.748082	4.822106
3.017208	205.550921	4.827110
3.077322	215.339749	4.832115
2.832229	213.653929	4.837120
3.134906	205.801508	4.842125
3.169549	212.566594	4.847130
3.223144	204.341910	4.852134
3.050438	203.075022	4.857139
2.619962	186.260617	4.862144
3.034862	202.590313	4.867149
2.880148	216.092270	4.872154
3.191465	208.092961	4.877158
3.298181	212.049977	4.882163
3.394234	215.704943	4.887168
3.431967	211.791804	4.892173
3.218457	208.186951	4.897178
2.849622	191.438815	4.902182
2.987367	213.215667	4.907187
3.191681	211.070289	4.912192
3.361915	214.982553	4.917197
3.008531	216.157934	4.922202
3.175819	213.325490	4.927206
3.580888	224.262509	4.932211
3.361776	210.661000	4.937216
3.506124	208.952127	4.942221
3.304044	219.962127	4.947226
3.512005	211.165920	4.952230
3.042423	198.894485	4.957235
3.339834	210.142594	4.962240
3.224812	217.927721	4.967245
3.393749	214.367349	4.972250
3.484071	216.849452	4.977254
3.583757	224.803423	4.982259
3.210776	220.413627	4.987264
3.370911	216.041544	4.992269
3.156125	216.059414	4.997274
3.091824	209.561639	5.002278
3.151902	221.134845	5.007283
3.000622	217.276629	5.012288
3.502400	212.110695	5.017293
3.046435	212.865547	5.022298
3.477944	213.323160	5.027302
3.244097	220.839002	5.032307
3.080956	221.858025	5.037312
3.524367	235.987623	5.042317
3.329480	239.893824	5.047322
3.657562	237.555042	5.052326
3.575965	241.022711	5.057331
3.668750	240.720305	5.062336
3.962878	243.116694	5.067341
3.710871	240.052546	5.072346
3.287777	221.319702	5.077350
3.636625	235.698235	5.082355
3.643797	237.443553	5.087360
3.821951	245.644668	5.092365
3.424230	246.406215	5.097370
3.385772	234.051388	5.102374
3.187951	240.397322	5.107379
3.363970	239.591489	5.112384
3.477581	241.538432	5.117389
3.712670	245.943582	5.122394
3.818799	244.863958	5.127398
3.902779	243.541031	5.132403
3.875895	245.298013	5.137408
3.877766	245.224989	5.142413
3.704126	249.466388	5.147418
3.798416	241.013846	5.152422
3.955190	248.718435	5.157427
3.802722	250.232501	5.162432
3.810341	241.875797	5.167437
3.913202	246.475673	5.172442
3.873139	240.755542	5.177446
3.815835	241.036642	5.182451
3.795109	237.331975	5.187456
4.014657	242.410280	5.192461
3.616086	246.797653	5.197466
3.731653	241.619455	5.202470
3.972303	233.403415	5.207475
3.674208	245.421900	5.212480
4.208290	238.184947	5.217485
3.915306	244.691328	5.222490
4.222466	237.727213	5.227494
3.931418	240.148850	5.232499
4.138581	233.377576	5.237504
4.047951	231.781449	5.242509
3.993581	235.830149	5.247514
4.188080	229.117810	5.252518
4.090888	239.361572	5.257523
4.089895	242.231312	5.262528
4.333777	239.545051	5.267533
3.861160	238.907287	5.272538
3.935586	243.201567	5.277542
3.867569	249.489202	5.282547
3.844549	254.010725	5.287552
3.810716	262.172295	5.292557
4.114030	262.472824	5.297562
4.223836	270.102523	5.302566
3.770044	268.433577	5.307571
3.915577	261.785846	5.312576
3.994065	265.449901	5.317581
4.095181	268.616862	5.322586
4.271753	265.207146	5.327590
4.424727	266.379124	5.332595
4.069075	262.663653	5.337600
4.690297	265.745958	5.342605
4.394356	264.245271	5.347610
4.459597	263.994637	5.352614
4.166116	266.783658	5.357619
4.085779	272.655611	5.362624
4.330298	268.909379	5.367629
3.943419	273.253797	5.372634
4.275603	264.855720	5.377638
4.249827	266.324627	5.382643
4.424166	258.172749	5.387648
4.279751	257.929654	5.392653
4.415715	268.064134	5.397658
4.687941	262.443765	5.402662
4.182890	271.849771	5.407667
4.437619	270.598166	5.412672
4.536240	282.608302	5.417677
4.411837	284.741240	5.422682
4.763455	276.450845	5.427686
4.504377	275.320873	5.432691
4.279797	270.724313	5.437696
4.304343	264.491010	5.442701
4.297406	290.599702	5.447706
4.918247	289.518525	5.452710
4.289009	285.820604	5.457715
4.643223	291.396685	5.462720
4.900211	289.698630	5.467725
4.662290	296.148945	5.472730
4.802516	292.621531	5.477734
4.872591	295.125800	5.482739
4.408901	280.271733	5.487744
4.778023	284.728659	5.492749
4.694418	290.711863	5.497754
4.751363	279.427236	5.502758
4.330326	280.989712	5.507763
4.955216	288.943679	5.512768
4.921486	285.332790	5.517773
4.539307	271.924465	5.522778
5.093175	279.513065	5.527782
4.805977	270.376792	5.532787
4.455042	272.431325	5.537792
4.591620	272.558660	5.542797
4.633628	280.869709	5.547802
5.197967	285.077747	5.552806
4.967008	290.239307	5.557811
4.815162	284.511367	5.562816
4.758113	277.857405	5.567821
4.712294	295.426809	5.572826
4.779970	284.953591	5.577830
4.808036	283.671058	5.582835
4.652266	285.362817	5.587840
4.873294	285.771152	5.592845
4.950961	294.503732	5.597850
5.007704	290.692002	5.602854
5.077454	295.129397	5.607859
4.661067	294.884622	5.612864
5.139808	287.403217	5.617869
4.821008	286.861574	5.622874
5.110144	285.968412	5.627878
4.734725	280.882950	5.632883
4.863456	283.213511	5.637888
5.075333	280.937224	5.642893
5.052246	296.301071	5.647898
5.316575	290.201035	5.652902
4.913695	289.495393	5.657907
4.579239	280.863234	5.662912
5.232318	287.262528	5.667917
5.060284	281.436511	5.672922
5.365608	289.712635	5.677926
5.147792	285.507322	5.682931
5.128323	285.282615	5.687936
4.970680	286.009711	5.692941
5.128985	296.007828	5.697946
4.852945	287.040642	5.702950
4.953209	289.340862	5.707955
4.707730	297.203411	5.712960
4.753984	297.879578	5.717965
5.203096	323.530881	5.722970
5.417626	317.232991	5.727974
5.352789	319.729928	5.732979
5.130921	318.701691	5.737984
5.584583	314.694887	5.742989
5.270312	325.010676	5.747994
5.483601	314.986031	5.752998
5.119830	332.858392	5.758003
5.469952	323.280545	5.763008
5.420127	321.450223	5.768013
5.426859	316.795263	5.773018
5.522174	312.290942	5.778022
5.218766	318.011197	5.783027
5.179954	315.998814	5.788032
5.231743	321.024332	5.793037
5.343509	323.022193	5.798042
5.562811	318.102970	5.803046
5.543398	315.625633	5.808051
5.368340	308.135925	5.813056
5.347954	311.245999	5.818061
5.454037	313.687681	5.823066
5.701086	308.096552	5.828070
5.700715	318.075249	5.833075
5.544218	312.439779	5.838080
5.292009	315.772840	5.843085
5.362496	321.519937	5.848090
5.634068	312.068300	5.853094
5.663690	315.170539	5.858099
5.504597	319.868425	5.863104
5.654532	309.986589	5.868109
5.538685	315.778698	5.873114
5.513918	312.017700	5.878118
5.636392	314.229021	5.883123
5.715081	325.201421	5.888128
5.938898	317.892825	5.893133
5.699539	317.152071	5.898138
5.826305	315.705374	5.903142
5.347642	316.871916	5.908147
5.471326	317.947245	5.913152
5.506466	317.938611	5.918157
5.505552	321.507550	5.923162
5.695693	327.153643	5.928166
5.575531	315.450647	5.933171
5.624767	320.226625	5.938176
5.723217	319.518364	5.943181
5.516295	326.716816	5.948186
5.759837	338.419542	5.953190
5.937624	348.645593	5.958195
5.771242	340.936210	5.963200
6.154771	337.785124	5.968205
5.789850	328.189592	5.973210
5.577079	320.958892	5.978214
6.054466	332.251647	5.983219
5.817026	336.667580	5.988224
6.126787	335.002382	5.993229
5.568191	324.285576	5.998234
5.748299	326.655548	6.003238
5.886707	330.835419	6.008243
5.919852	342.523656	6.013248
5.634451	338.142256	6.018253
5.722071	332.753272	6.023258
5.827814	338.017117	6.028262
5.674387	347.871114	6.033267
6.138157	345.922352	6.038272
6.077695	345.235826	6.043277
5.797182	343.713732	6.048282
6.072233	339.298304	6.053286
5.810132	334.786701	6.058291
5.620244	332.544883	6.063296
5.929437	327.089546	6.068301
5.688834	344.898329	6.073306
6.040681	338.512477	6.078310
6.562838	333.507832	6.083315
5.594414	331.020995	6.088320
5.781511	323.268891	6.093325
5.458577	333.348757	6.098330
6.008484	337.729914	6.103334
5.879889	342.676132	6.108339
5.907996	343.026109	6.113344
6.037500	342.528121	6.118349
5.464952	330.804245	6.123354
5.919508	334.649840	6.128358
6.291762	342.700364	6.133363
5.635381	332.887901	6.138368
6.037200	331.489857	6.143373
5.427478	328.798121	6.148378
5.907561	342.836636	6.153382
6.176910	346.828313	6.158387
5.967705	344.029527	6.163392
6.072065	321.436359	6.168397
5.836882	320.694950	6.173402
5.804479	327.280757	6.178406
5.627222	326.115814	6.183411
5.578093	330.603483	6.188416
5.868532	339.742515	6.193421
6.095576	349.106623	6.198426
6.014224	339.017396	6.203430
5.936234	333.341144	6.208435
5.803330	325.063366	6.213440
6.242630	318.518284	6.218445
5.815811	314.934177	6.223450
6.207951	310.408659	6.228454
5.833717	319.651823	6.233459
5.422793	322.399141	6.238464
5.803985	318.353070	6.243469
5.465552	315.530243	6.248474
6.108692	317.830830	6.253478
5.853997	317.994160	6.258483
5.727300	314.862908	6.263488
5.938516	324.403492	6.268493
5.748286	318.561330	6.273498
5.782168	313.142806	6.278502
6.164461	330.882453	6.283507
5.844374	320.492116	6.288512
5.795369	323.445323	6.293517
5.739523	318.025037	6.298522
5.760265	320.897712	6.303526
5.938297	326.137572	6.308531
6.121043	340.149904	6.313536
6.144364	317.521982	6.318541
5.778592	324.188494	6.323546
5.847947	312.284961	6.328550
5.874439	317.365062	6.333555
5.977753	319.133290	6.338560
5.912869	314.442095	6.343565
5.510017	322.674166	6.348570
5.731252	316.030372	6.353574
5.713770	318.257294	6.358579
5.653239	324.347627	6.363584
6.334643	327.214867	6.368589
5.819505	328.089728	6.373594
5.620586	316.285175	6.378598
5.829213	327.575744	6.383603
5.805496	334.134882	6.388608
5.832399	322.760020	6.393613
6.192845	337.079870	6.398618
5.705674	322.710343	6.403622
5.677352	335.480733	6.408627
5.853047	337.683718	6.413632
5.871233	329.822033	6.418637
5.766470	332.290425	6.423642
6.059555	334.209258	6.428646
5.830841	336.592666	6.433651
5.547089	324.845692	6.438656
6.190595	330.911140	6.443661
5.808759	333.299557	6.448666
5.932644	323.909019	6.453670
5.850801	324.225602	6.458675
5.545664	325.909130	6.463680
6.011807	333.777257	6.468685
6.150394	353.016784	6.473690
5.956966	331.941428	6.478694
5.799869	328.147376	6.483699
5.563493	326.368429	6.488704
5.827094	325.150231	6.493709
5.614512	342.170000	6.498714
6.036664	344.650750	6.503718
6.077207	346.897058	6.508723
5.757386	337.044515	6.513728
6.016470	320.020701	6.518733
5.772650	320.707517	6.523738
6.026208	321.373351	6.528742
5.662670	323.145123	6.533747
5.711889	326.029156	6.538752
6.019176	331.881525	6.543757
5.806566	339.960409	6.548762
5.648953	349.191794	6.553766
6.357483	350.488707	6.558771
5.559379	342.084189	6.563776
6.019516	329.413889	6.568781
5.483519	326.609361	6.573786
5.979223	340.670736	6.578790
6.023131	346.466299	6.583795
5.693844	343.768587	6.588800
5.923077	350.468434	6.593805
5.975055	344.835091	6.598810
5.717647	337.364601	6.603814
6.250081	336.003040	6.608819
5.594003	329.439752	6.613824
5.780151	326.582188	6.618829
6.284915	344.584237	6.623834
5.747037	332.048160	6.628838
5.546156	324.594129	6.633843
5.821278	335.241525	6.638848
6.288985	332.488544	6.643853
6.196323	333.240263	6.648858
5.892552	312.489107	6.653862
5.975957	326.023441	6.658867
5.623776	323.712138	6.663872
5.954820	316.529113	6.668877
5.487272	320.949458	6.673882
5.705132	324.053844	6.678886
5.847982	334.981396	6.683891
5.392055	328.367765	6.688896
6.045274	333.637579	6.693901
5.958838	347.850284	6.698906
5.879091	342.690003	6.703910
6.058649	338.666029	6.708915
5.715487	336.732967	6.713920
5.790353	331.583266	6.718925
5.949762	342.157047	6.723930
6.082803	329.873359	6.728934
5.980944	321.609702	6.733939
6.051283	320.801441	6.738944
5.901728	320.340849	6.743949
5.401511	325.854659	6.748954
5.851160	321.310637	6.753958
5.939656	320.164168	6.758963
5.895457	328.498238	6.763968
5.925678	320.337275	6.768973
5.725081	321.308387	6.773978
5.437152	320.698631	6.778982
5.924491	329.648617	6.783987
5.949950	338.721597	6.788992
6.150618	342.803130	6.793997
5.857374	330.978544	6.799002
5.949323	323.140106	6.804006
5.795874	315.049053	6.809011
5.638391	318.452695	6.814016
5.914541	319.121317	6.819021
5.604018	331.575247	6.824026
5.770657	338.183655	6.829030
6.038335	349.158098	6.834035
5.974503	357.568024	6.839040
5.843203	349.935399	6.844045
5.513077	344.845986	6.849050
5.941415	344.592245	6.854054
6.261347	349.996543	6.859059
5.819867	341.254571	6.864064
6.211121	326.510123	6.869069
5.596995	333.696448	6.874074
5.619495	320.847949	6.879078
6.229591	333.341136	6.884083
5.593185	330.479572	6.889088
5.907891	324.703829	6.894093
5.579346	325.875325	6.899098
5.950971	336.896749	6.904102
5.480494	344.604744	6.909107
5.517515	341.476310	6.914112
6.009341	357.297379	6.919117
6.214773	365.557551	6.924122
6.132818	351.535806	6.929126
5.897033	351.784759	6.934131
5.574111	340.638706	6.939136
6.379689	344.859582	6.944141
6.046622	342.652851	6.949146
5.756145	330.005245	6.954150
6.185360	333.351767	6.959155
5.942038	328.331016	6.964160
6.009785	323.925925	6.969165
5.694569	328.420482	6.974170
5.728344	327.712863	6.979174
6.028641	334.053553	6.984179
5.518232	327.185864	6.989184
5.764125	332.044929	6.994189
5.567118	327.551604	6.999194
5.695737	331.391318	7.004198
5.906005	337.046916	7.009203
5.789386	354.662273	7.014208
6.020309	349.200210	7.019213
5.889565	341.741511	7.024218
6.175382	335.925997	7.029222
6.100722	331.726717	7.034227
5.703029	330.067959	7.039232
6.060134	326.870394	7.044237
5.676518	328.964856	7.049242
5.786070	326.182569	7.054246
5.809063	320.699310	7.059251
5.470386	325.646801	7.064256
5.946244	334.642882	7.069261
5.712056	339.836600	7.074266
5.694998	342.284924	7.079270
6.092201	337.271382	7.084275
5.941412	348.915675	7.089280
5.836147	337.612133	7.094285
5.706530	343.532961	7.099290
5.978674	348.786556	7.104294
5.757540	341.364166	7.109299
5.983207	355.195776	7.114304
5.944480	338.879840	7.119309
5.776039	341.712556	7.124314
5.880755	345.176363	7.129318
6.015311	346.351233	7.134323
6.017844	338.314824	7.139328
5.916237	326.763939	7.144333
5.612024	342.231986	7.149338
5.997589	330.724992	7.154342
5.537387	325.165577	7.159347
5.986300	326.376613	7.164352
5.921142	328.016213	7.169357
5.594922	330.962235	7.174362
6.185110	332.518137	7.179366
5.672878	332.506680	7.184371
5.632168	335.360511	7.189376
5.892746	335.477909	7.194381
5.794573	344.041908	7.199386
5.908381	357.802460	7.204390
6.010324	350.965370	7.209395
6.130549	348.466150	7.214400
5.783030	327.193476	7.219405
5.787123	334.453783	7.224410
5.656551	334.148406	7.229414
6.080961	339.821073	7.234419
5.210990	342.165748	7.239424
6.015992	344.535892	7.244429
6.113718	349.345410	7.249434
5.935610	349.667585	7.254438
6.248954	343.835101	7.259443
5.937293	336.721129	7.264448
6.011247	328.683026	7.269453
5.402480	336.074159	7.274458
5.619358	331.933606	7.279462
5.786076	341.167955	7.284467
5.860425	356.111621	7.289472
6.076951	347.108358	7.294477
5.681745	348.397870	7.299482
5.867751	346.040206	7.304486
6.156420	351.224773	7.309491
5.625596	347.280462	7.314496
6.015169	339.537756	7.319501
5.975459	337.607770	7.324506
5.741602	339.998312	7.329510
5.796402	331.504457	7.334515
5.881555	347.325959	7.339520
6.141164	330.536174	7.344525
5.834244	333.428552	7.349530
5.722328	324.720373	7.354534
6.099974	334.620869	7.359539
5.638126	329.783056	7.364544
6.056464	323.614584	7.369549
5.941008	326.268151	7.374554
5.947840	320.129354	7.379558
6.054975	328.177117	7.384563
5.689072	328.468604	7.389568
5.749055	321.815272	7.394573
5.535522	342.451407	7.399578
5.571747	329.777923	7.404582
5.737926	335.807428	7.409587
5.829957	344.509308	7.414592
6.007442	343.560869	7.419597
5.932479	356.028529	7.424602
5.922567	347.826385	7.429606
6.247709	346.022732	7.434611
5.554601	335.140331	7.439616
5.654475	335.010822	7.444621
5.774865	345.672976	7.449626
6.070614	344.832560	7.454630
6.210497	338.353367	7.459635
5.703027	330.532913	7.464640
5.941232	321.001076	7.469645
5.860064	331.103173	7.474650
5.940978	321.779481	7.479654
5.572830	323.349493	7.484659
5.727861	325.976498	7.489664
6.186720	331.495067	7.494669
5.997207	329.145621	7.499674
5.744954	333.848616	7.504678
5.728893	325.951169	7.509683
5.851712	329.614620	7.514688
5.831311	331.041560	7.519693
6.181040	334.457485	7.524698
5.907519	332.013632	7.529702
6.079456	331.240073	7.534707
5.884811	338.724511	7.539712
5.791402	322.768339	7.544717
5.929877	327.027293	7.549722
5.946317	317.305576	7.554726
5.850380	322.252999	7.559731
5.965083	337.221964	7.564736
5.923266	336.722345	7.569741
5.964260	323.719083	7.574746
5.893434	319.990610	7.579750
6.018793	323.283498	7.584755
5.563981	329.859558	7.589760
6.009873	321.693578	7.594765
6.070814	329.400562	7.599770
6.114380	328.814797	7.604774
6.027375	322.535676	7.609779
6.139105	317.111281	7.614784
6.417095	321.595151	7.619789
6.115959	325.767958	7.624794
6.113913	302.691606	7.629798
6.057161	298.011795	7.634803
6.008091	301.309862	7.639808
5.817860	300.396893	7.644813
5.601938	300.538329	7.649818
5.432842	304.253840	7.654822
6.003573	302.319962	7.659827
5.340425	309.257691	7.664832
5.870341	314.214621	7.669837
5.869754	331.906690	7.674842
5.787025	324.143077	7.679846
6.044244	321.555957	7.684851
6.223636	323.432490	7.689856
6.029734	305.017991	7.694861
5.916590	306.475280	7.699866
5.669310	298.234418	7.704870
5.462493	306.508534	7.709875
5.702541	320.059451	7.714880
5.708412	322.478869	7.719885
5.730794	320.573958	7.724890
6.072034	324.478435	7.729894
5.827715	321.451033	7.734899
6.152346	329.021788	7.739904
6.378518	315.932570	7.744909
5.937900	306.965850	7.749914
5.631793	302.236522	7.754918
5.588010	295.175509	7.759923
5.507824	312.095410	7.764928
5.970482	312.370973	7.769933
5.686737	328.661551	7.774938
5.610020	323.652664	7.779942
5.862713	320.908062	7.784947
6.143232	331.684327	7.789952
6.223131	315.182144	7.794957
5.943992	330.184338	7.799962
5.875961	322.364639	7.804966
5.948234	308.049841	7.809971
5.803237	311.109836	7.814976
5.898975	305.972691	7.819981
5.511948	314.249736	7.824986
5.880020	325.094537	7.829990
6.129830	325.118708	7.834995
5.904609	316.874381	7.840000
6.006741	308.803398	7.845005
5.439652	310.575424	7.850010
5.692719	307.511223	7.855014
6.110477	313.852484	7.860019
6.276683	316.616944	7.865024
5.834516	301.114073	7.870029
5.667737	307.047039	7.875034
5.720477	307.813940	7.880038
5.921143	301.834607	7.885043
5.422207	309.284452	7.890048
5.976885	314.613993	7.895053
6.195774	318.445889	7.900058
5.957093	310.567511	7.905062
5.828781	308.524858	7.910067
5.662720	300.815442	7.915072
5.904106	312.119851	7.920077
6.005913	324.398439	7.925082
6.364420	316.043671	7.930086
6.275842	307.129362	7.935091
5.748814	310.796549	7.940096
5.893409	302.174743	7.945101
5.425455	308.907881	7.950106
5.876273	295.384841	7.955110
5.685133	293.291922	7.960115
5.892320	302.750867	7.965120
5.717412	301.601377	7.970125
5.417029	306.503606	7.975142
5.715605	307.476159	7.980160
5.880767	317.668545	7.985178
5.996062	322.289430	7.990195
6.049198	319.220088	7.995213
6.088693	317.370994	8.000230
6.048830	312.754142	8.005248
5.845209	310.971541	8.010266
5.847516	304.893296	8.015283
5.873505	302.074357	8.020301
5.673133	304.687167	8.025318
5.532633	314.867485	8.030336
6.083303	323.450012	8.035354
6.056146	334.433071	8.040371
6.027339	326.286382	8.045389
6.245791	330.723852	8.050406
5.896955	319.894451	8.055424
5.974213	305.321880	8.060442
5.635977	307.899488	8.065459
6.134994	315.549700	8.070477
5.792225	328.046460	8.075494
5.723583	327.798482	8.080512
5.676350	320.620334	8.085530
5.998896	321.500772	8.090547
5.791632	330.848981	8.095565
5.984058	324.535819	8.100582
5.920719	324.577336	8.105600
6.200797	317.262702	8.110618
5.967202	326.299462	8.115635
5.696524	329.185216	8.120653
5.855051	327.658288	8.125670
5.634176	325.565973	8.130688
5.839720	323.135453	8.135706
5.696694	335.162277	8.140723
5.845548	323.929854	8.145741
5.846172	323.992907	8.150758
5.924260	329.547406	8.155776
6.409678	329.793270	8.160794
6.033805	329.034865	8.165811
6.110268	335.062979	8.170829
6.184321	323.267935	8.175846
5.902393	321.740593	8.180864
6.041690	324.921864	8.185882
5.989053	329.404965	8.190899
6.309246	323.885961	8.195917
6.047727	328.960353	8.200934
5.960425	329.504229	8.205952
6.211156	318.511462	8.210970
5.805680	321.210057	8.215987
6.259442	334.358328	8.221005
6.270418	331.447065	8.226022
5.921751	327.544452	8.231040
6.268893	326.653830	8.236058
5.852689	339.061120	8.241075
6.153011	346.155512	8.246093
6.668183	347.131999	8.251110
6.155117	336.236803	8.256128
6.255218	329.590976	8.261146
5.805963	334.833636	8.266163
6.087380	338.510180	8.271181
6.287686	342.925251	8.276198
6.154879	333.873381	8.281216
6.427715	325.023040	8.286234
6.076791	324.352242	8.291251
6.145060	323.057202	8.296269
6.289078	322.779059	8.301286
6.150756	335.221701	8.306304
6.529469	326.301123	8.311322
6.282708	337.104001	8.316339
6.698627	327.893578	8.321357
6.701665	331.033084	8.326374
6.290892	334.070174	8.331392
6.419796	327.707005	8.336410
6.265401	334.276206	8.341427
6.531136	326.812340	8.346445
6.007966	324.376079	8.351462
6.214456	339.705834	8.356480
6.321896	321.587795	8.361498
6.111036	332.574389	8.366515
6.296237	319.565913	8.371533
6.268541	322.012818	8.376550
5.924673	329.444815	8.381568
6.303241	318.037553	8.386586
6.105556	325.102670	8.391603
6.172546	326.578556	8.396621
6.001609	330.559498	8.401638
5.985437	329.397605	8.406656
6.123651	324.705513	8.411674
6.061136	334.419199	8.416691
6.612885	341.489974	8.421709
6.475921	334.982271	8.426726
6.240500	328.445816	8.431744
6.380594	329.392710	8.436762
6.319947	331.952074	8.441779
6.368873	326.194713	8.446797
6.231799	322.899560	8.451814
6.507218	342.418786	8.456832
6.268509	326.437758	8.461850
6.350819	342.345535	8.466867
6.112723	344.576106	8.471885
6.513216	349.982270	8.476902
6.165947	355.672848	8.481920
6.534750	350.338720	8.486938
6.554501	357.858921	8.491955
6.390728	358.405312	8.496973
6.547026	352.151449	8.501990
6.313717	363.176292	8.507008
6.380265	348.662167	8.512026
6.390057	356.022984	8.517043
6.558028	363.803980	8.522061
6.651966	351.115885	8.527078
6.131462	357.445819	8.532096
6.541443	354.131217	8.537114
6.516212	357.843188	8.542131
6.380824	353.525308	8.547149
6.629831	347.263232	8.552166
6.421748	355.257775	8.557184
6.372146	355.164599	8.562202
6.187451	355.259844	8.567219
5.956819	354.311428	8.572237
6.413922	351.806777	8.577255
6.635373	362.419548	8.582272
6.412393	350.652091	8.587290
6.256602	356.167506	8.592307
6.264620	353.619611	8.597325
6.732138	346.518588	8.602343
6.242734	360.925471	8.607360
6.354085	362.754163	8.612378
6.286088	359.293549	8.617395
6.469530	362.619385	8.622413
6.344545	361.417736	8.627431
6.361404	363.403240	8.632448
6.662398	379.194738	8.637466
6.901226	381.969112	8.642483
6.820052	371.754135	8.647501
6.759365	367.131064	8.652519
6.506990	364.810155	8.657536
6.763661	363.299405	8.662554
6.495337	362.543082	8.667571
6.450313	352.653803	8.672589
6.542339	357.246785	8.677607
6.597275	359.548208	8.682624
6.569912	353.853283	8.687642
6.797355	361.883729	8.692659
6.819296	361.394345	8.697677
6.587892	362.200635	8.702695
6.541449	358.780824	8.707712
6.655872	362.155343	8.712730
6.658488	370.410363	8.717747
6.517654	366.304767	8.722765
6.802110	353.012478	8.727783
6.691852	374.264704	8.732800
6.088381	360.906407	8.737818
6.459974	372.846313	8.742835
6.533827	385.375664	8.747853
7.022501	383.172169	8.752871
6.477844	381.200003	8.757888
6.977526	377.700933	8.762906
6.914345	380.841356	8.767923
6.839409	378.656742	8.772941
7.258913	370.821635	8.777959
6.469944	377.499745	8.782976
6.455272	358.173222	8.787994
6.621993	368.239163	8.793011
6.787299	367.894570	8.798029
7.172777	374.495960	8.803047
6.477092	374.462988	8.808064
6.676003	373.125385	8.813082
6.901857	386.255756	8.818099
6.780964	385.842398	8.823117
6.604421	376.895186	8.828135
6.695341	382.419290	8.833152
6.466470	384.569528	8.838170
6.627434	382.654059	8.843187
6.492298	388.084197	8.848205
7.057383	380.873201	8.853223
6.923729	385.261715	8.858240
7.012170	382.073225	8.863258
7.083443	383.740944	8.868275
7.037665	382.621555	8.873293
7.088950	374.282419	8.878311
6.731309	387.043476	8.883328
6.911108	382.490017	8.888346
7.338812	383.675866	8.893363
7.127031	373.860039	8.898381
6.873018	364.988086	8.903399
6.506204	361.703676	8.908416
6.445464	361.672204	8.913434
6.745888	372.837484	8.918451
6.999395	377.869063	8.923469
6.894846	378.942651	8.928487
6.728056	388.940941	8.933504
6.999179	377.108673	8.938522
6.912136	380.341195	8.943539
6.772337	382.707845	8.948557
7.377921	387.419182	8.953575
7.324538	380.150458	8.958592
7.001552	376.145981	8.963610
7.317810	372.732454	8.968627
6.895352	358.979733	8.973645
7.082115	363.567340	8.978663
6.502603	364.021084	8.983680
7.096684	376.143878	8.988698
6.788232	362.297554	8.993715
7.094170	367.775341	8.998733
6.963995	371.188185	9.003751
6.729440	377.015741	9.008768
6.639132	388.485243	9.013786
7.006072	382.179431	9.018803
7.063620	380.538935	9.023821
7.025446	374.678443	9.028839
6.990018	382.336685	9.033856
6.812906	385.636968	9.038874
7.340016	374.701846	9.043891
7.208780	380.876124	9.048909
7.277706	379.975444	9.053927
7.115743	375.191518	9.058944
6.684029	372.901863	9.063962
7.135121	374.945562	9.068979
6.627206	385.145618	9.073997
7.248205	381.883153	9.079015
7.125905	379.797476	9.084032
6.848455	386.827780	9.089050
6.995163	375.829185	9.094067
7.029784	383.302886	9.099085
6.837927	380.205650	9.104103
7.199716	385.056167	9.109120
6.870356	382.693670	9.114138
7.059109	379.457906	9.119155
7.405917	385.434212	9.124173
7.599140	382.443895	9.129191
7.113081	376.912348	9.134208
6.828213	384.253074	9.139226
7.319634	381.253903	9.144243
7.227077	388.678107	9.149261
7.029817	385.919379	9.154279
7.145215	379.226956	9.159296
6.972856	382.204609	9.164314
7.081503	381.966720	9.169331
6.981947	381.600511	9.174349
7.141985	380.041785	9.179367
7.267000	388.293414	9.184384
7.033237	394.243926	9.189402
7.409996	398.419929	9.194419
7.099158	411.561827	9.199437
7.369347	399.250018	9.204455
7.525753	415.423955	9.209472
7.074551	402.123819	9.214490
7.434324	390.501709	9.219507
7.244026	394.539347	9.224525
7.264013	388.985311	9.229543
7.111747	390.653342	9.234560
6.936047	405.440290	9.239578
7.529486	404.750910	9.244595
7.274722	404.642543	9.249613
7.456374	405.355716	9.254631
7.479310	407.576954	9.259648
7.339826	408.671796	9.264666
7.289053	401.948597	9.269683
6.756298	408.854812	9.274701
7.155204	400.136156	9.279719
7.395580	403.661358	9.284736
7.361200	403.669936	9.289754
7.487003	400.734359	9.294771
7.412957	400.398866	9.299789
7.634254	398.079474	9.304807
7.294835	399.600109	9.309824
7.242935	401.324998	9.314842
7.410083	401.141058	9.319859
7.226603	407.348777	9.324877
7.423640	409.975073	9.329895
7.441086	409.076146	9.334912
7.408824	407.411850	9.339930
7.418800	398.170322	9.344947
7.171545	402.696557	9.349965
7.408485	409.889266	9.354983
7.641896	411.111871	9.360000
7.682207	408.486327	9.365018
7.823387	400.215143	9.370035
7.371256	399.026880	9.375053
7.569559	399.974124	9.380071
7.282940	406.115954	9.385088
7.420952	409.092317	9.390106
7.555863	402.251664	9.395123
7.465484	414.503817	9.400141
7.439860	416.439181	9.405159
7.470420	408.109587	9.410176
7.730954	411.691591	9.415194
8.046401	402.853469	9.420211
7.662442	399.679033	9.425229
7.358226	399.786693	9.430247
7.744010	404.071734	9.435264
7.348924	405.635804	9.440282
7.529554	410.101311	9.445299
7.433735	404.183571	9.450317
7.557174	408.964145	9.455335
7.578892	411.485369	9.460352
7.713336	406.860117	9.465370
7.860511	404.113691	9.470387
7.529950	404.364331	9.475405
7.657459	411.047178	9.480423
7.490470	402.855834	9.485440
7.459753	411.772489	9.490458
7.376268	411.305933	9.495475
7.344320	413.286468	9.500493
7.351114	411.903225	9.505511
7.535307	410.952925	9.510528
7.743214	408.925959	9.515546
7.449400	409.590555	9.520563
7.378158	411.766590	9.525581
7.714061	410.076167	9.530599
7.594751	410.981660	9.535616
7.420677	411.621183	9.540634
7.760067	416.415260	9.545651
7.827348	428.418662	9.550669
7.436881	426.084668	9.555687
7.852419	429.389930	9.560704
7.765106	436.791241	9.565722
7.701401	425.812961	9.570739
7.603982	439.328531	9.575757
8.020672	431.572731	9.580775
8.092414	427.604225	9.585792
7.744538	415.704818	9.590810
7.747891	418.427733	9.595827
7.643451	410.526380	9.600845
7.529367	405.892732	9.605863
7.769348	421.103703	9.610880
7.794983	422.197920	9.615898
8.159598	428.449156	9.620915
7.686644	424.474477	9.625933
7.532028	425.073084	9.630951
7.966326	422.259578	9.635968
7.667894	436.646067	9.640986
7.907318	433.531740	9.646003
7.947072	422.837047	9.651021
7.759086	429.083349	9.656039
7.872275	426.597859	9.661056
7.611191	429.942865	9.666074
7.754758	424.801792	9.671091
7.823040	431.383476	9.676109
7.944340	443.435227	9.681127
7.860407	435.319216	9.686144
7.814232	437.343007	9.691162
7.709962	431.237237	9.696179
7.811341	436.990088	9.701197
7.707107	436.795021	9.706215
8.174143	430.025393	9.711232
7.357231	431.917484	9.716250
7.784992	436.836573	9.721267
8.049907	439.774124	9.726285
7.522012	437.382768	9.731303
7.965592	433.946124	9.736320
7.643383	436.290870	9.741338
8.029257	447.445964	9.746355
8.179532	440.208421	9.751373
7.803087	441.229941	9.756391
8.009916	439.865846	9.761408
8.334029	448.300899	9.766426
8.022279	438.696355	9.771443
7.930842	435.548662	9.776461
7.673855	439.457905	9.781479
8.079357	438.485552	9.786496
7.674724	459.569412	9.791514
8.024048	449.195422	9.796531
8.136026	457.461749	9.801549
8.131591	459.952365	9.806567
8.298064	455.779665	9.811584
8.145040	457.040730	9.816602
8.311087	448.166035	9.821619
8.306350	451.688626	9.826637
8.018365	443.898066	9.831655
8.285992	430.519995	9.836672
7.631754	436.659475	9.841690
8.125216	449.022142	9.846707
8.048230	446.235094	9.851725
7.780316	447.220675	9.856743
8.336734	443.040528	9.861760
8.544622	456.432537	9.866778
8.584336	450.089610	9.871795
8.271218	450.056657	9.876813
8.204378	435.096310	9.881831
8.358359	431.127541	9.886848
8.188141	433.880809	9.891866
7.879470	438.839545	9.896883
8.266266	430.207978	9.901901
8.060540	434.980173	9.906919
8.438135	445.177217	9.911936
8.289966	437.367910	9.916954
8.010428	434.044565	9.921971
8.388242	442.095668	9.926989
8.320820	443.677828	9.932007
8.248057	435.010967	9.937024
8.316712	432.731267	9.942042
8.302800	432.389506	9.947059
7.874566	423.775190	9.952077
8.084145	450.446296	9.957095
8.444095	453.640354	9.962112
8.441030	453.606156	9.967130
8.289798	450.000779	9.972147
8.506889	449.900530	9.977165
8.104812	443.869818	9.982183
8.287510	441.423928	9.987200
8.490436	446.157345	9.992218
8.779623	443.915672	9.997235
8.423952	439.698556	10.002253
7.938708	437.660271	10.007271
8.497294	443.669686	10.012288
8.615694	448.277494	10.017306
8.650870	441.824830	10.022323
8.288245	434.001789	10.027341
8.211349	433.811906	10.032359
8.529605	430.252890	10.037376
8.175563	439.867146	10.042394
8.261600	446.187282	10.047411
8.579960	444.767843	10.052429
8.313764	446.160246	10.057447
8.807052	440.503635	10.062464
8.241041	444.063674	10.067482
8.375709	441.341292	10.072499
8.405484	443.340561	10.077517
8.299171	443.029056	10.082535
8.721071	442.372864	10.087552
8.224845	453.751376	10.092570
8.261916	458.460290	10.097587
8.531967	449.206388	10.102605
8.004933	464.528106	10.107623
8.274503	456.874240	10.112640
8.674669	457.603670	10.117658
8.286499	459.431744	10.122675
8.098698	448.005843	10.127693
8.249908	459.620582	10.132711
8.560871	449.284160	10.137728
8.322385	456.990027	10.142746
8.555012	466.190491	10.147763
8.845538	472.592203	10.152781
8.167717	470.142283	10.157799
8.638784	467.701700	10.162816
8.791380	475.690276	10.167834
8.369555	477.539404	10.172851
8.576595	471.694107	10.177869
8.510635	479.325616	10.182887
8.897975	472.170835	10.187904
8.649035	483.267628	10.192922
8.457220	471.324797	10.197939
8.856106	473.547098	10.202957
8.391663	476.898729	10.207975
8.711796	471.079894	10.212992
8.888705	476.795677	10.218010
8.869749	478.423895	10.223027
8.888240	477.357546	10.228045
8.615144	475.888766	10.233063
8.598819	470.760109	10.238080
8.563628	474.527313	10.243098
8.358074	477.245099	10.248115
8.752072	470.445876	10.253133
8.661339	481.483166	10.258151
9.146151	473.770323	10.263168
8.806387	482.596582	10.268186
8.699467	480.293892	10.273203
8.465078	479.377616	10.278221
8.473880	482.311122	10.283239
8.859093	474.497121	10.288256
8.556924	485.460246	10.293274
8.739709	481.559535	10.298291
8.954766	488.733614	10.303309
8.374668	484.365461	10.308327
8.552867	480.238255	10.313344
8.646195	482.656753	10.318362
8.807593	494.828487	10.323379
8.767219	490.804951	10.328397
8.698688	497.168257	10.333415
9.344540	500.178675	10.338432
8.918443	497.967017	10.343450
8.802757	487.564879	10.348467
9.029485	478.017954	10.353485
8.911401	478.819117	10.358503
8.823979	477.681001	10.363520
9.269257	478.330782	10.368538
8.785228	478.558132	10.373555
9.019755	475.627598	10.378573
8.869958	474.063762	10.383591
8.949614	470.930280	10.388608
8.801520	481.339096	10.393626
8.817590	494.089012	10.398643
9.233218	502.986271	10.403661
8.877323	492.381929	10.408679
9.326586	493.820024	10.413696
9.332467	496.615137	10.418714
8.820458	484.018733	10.423731
8.946895	475.115518	10.428749
8.869050	481.095276	10.433767
8.775524	482.766736	10.438784
9.028114	493.482002	10.443802
8.860445	501.388228	10.448819
9.015252	504.740667	10.453837
9.240201	507.725517	10.458855
9.171349	506.827483	10.463872
9.394706	501.459295	10.468890
8.931191	507.224939	10.473907
9.455713	500.408409	10.478925
8.921945	497.793905	10.483943
8.985931	502.930953	10.488960
9.131049	494.902101	10.493978
9.107506	505.704820	10.498995
9.270337	508.604730	10.504013
9.166710	508.046654	10.509031
8.969222	501.040296	10.514048
9.004194	493.287475	10.519066
9.405275	504.153049	10.524083
9.388707	502.928091	10.529101
9.338651	500.752187	10.534119
9.002945	507.015350	10.539136
9.284993	499.400536	10.544154
9.349373	509.302714	10.549171
9.348723	505.506476	10.554189
9.046711	509.107214	10.559207
9.003668	505.292372	10.564224
9.457985	504.956142	10.569242
8.913306	511.346721	10.574259
8.932211	495.353579	10.579277
9.287100	493.720134	10.584295
8.960327	496.217079	10.589312
9.376347	497.922310	10.594330
9.595840	506.692514	10.599347
9.557377	502.264739	10.604365
9.467479	508.426273	10.609383
9.474076	504.875050	10.614400
9.318534	506.897050	10.619418
8.942563	507.606079	10.624435
9.247038	496.150353	10.629453
9.163701	503.289141	10.634471
9.367958	501.944379	10.639488
9.549951	506.037318	10.644506
9.110581	503.669951	10.649523
9.375342	508.627222	10.654541
9.134117	507.497423	10.659559
9.066390	509.262671	10.664576
9.668316	504.857633	10.669594
9.032176	499.996492	10.674611
9.045007	506.407013	10.679629
9.124375	517.733250	10.684647
9.208670	525.401196	10.689664
9.459344	532.901067	10.694682
9.425738	533.711088	10.699699
9.569021	537.257840	10.704717
9.451287	525.824067	10.709735
9.276057	542.441395	10.714752
9.369611	530.737831	10.719770
9.242506	536.337168	10.724787
9.651344	529.125348	10.729805
9.261825	531.509053	10.734823
9.288702	537.810089	10.739840
9.391830	533.019300	10.744858
9.658254	532.087668	10.749875
9.176372	529.726958	10.754893
9.540726	538.856328	10.759911
9.344355	540.723785	10.764928
9.774846	550.871577	10.769946
9.824649	555.537497	10.774963
9.918328	534.612768	10.779981
9.458212	527.808492	10.784999
9.504266	544.457422	10.790016
9.781693	538.825135	10.795034
9.549112	541.338885	10.800051
9.809696	541.193952	10.805069
10.042365	540.703104	10.810087
9.764475	539.418104	10.815104
9.670872	539.104606	10.820122
9.739570	528.623062	10.825139
9.885052	536.956759	10.830157
9.790608	532.345247	10.835175
9.454201	541.290928	10.840192
9.574446	532.596934	10.845210
9.380476	531.156777	10.850227
9.966821	526.088310	10.855245
9.808113	531.878786	10.860263
9.576096	525.786688	10.865280
9.730485	527.627588	10.870298
9.451165	537.536297	10.875315
9.864745	551.173856	10.880333
10.204135	557.899299	10.885351
10.067231	544.859077	10.890368
9.770014	527.971864	10.895386
9.694560	532.158793	10.900403
9.951814	523.509608	10.905421
9.894608	523.244056	10.910439
9.821558	536.295140	10.915456
9.711977	522.225030	10.920474
10.024559	542.193082	10.925491
9.658084	538.646657	10.930509
10.039299	536.485226	10.935527
9.919648	548.536933	10.940544
10.143381	539.429095	10.945562
9.766861	529.269769	10.950579
9.965728	530.163284	10.955597
9.816723	535.557772	10.960615
10.146780	538.945874	10.965632
10.171782	529.985942	10.970650
10.160981	536.239233	10.975667
9.987707	526.729708	10.980685
9.872266	518.612284	10.985703
9.655513	522.152329	10.990720
9.793233	531.910487	10.995738
10.351329	549.163995	11.000755
9.908259	536.676671	11.005773
10.093238	545.266111	11.010791
10.128186	547.173064	11.015808
9.992168	549.450782	11.020826
10.389744	547.463510	11.025843
10.005162	538.902258	11.030861
9.898768	529.994471	11.035879
9.714320	538.133713	11.040896
10.459453	546.373460	11.045914
10.356107	547.816093	11.050931
9.955758	534.902361	11.055949
10.186533	534.566441	11.060967
9.806682	527.440325	11.065984
10.090632	547.210900	11.071002
10.132210	548.675007	11.076019
10.031377	560.685904	11.081037
10.577383	563.030331	11.086055
10.364026	548.241167	11.091072
10.367922	542.187839	11.096090
10.083205	534.690213	11.101107
9.910581	545.456355	11.106125
10.118337	542.242831	11.111143
10.067702	551.689689	11.116160
10.205050	552.368784	11.121178
10.219191	556.371270	11.126195
10.167195	556.578266	11.131213
10.323646	558.141139	11.136231
10.217434	558.053676	11.141248
10.322819	562.420559	11.146266
9.938247	561.316372	11.151283
10.502774	561.221646	11.156301
10.272544	550.916312	11.161319
10.037201	564.933262	11.166336
10.444690	557.005284	11.171354
10.419617	551.215264	11.176371
10.299617	555.633237	11.181389
10.422899	556.888886	11.186407
10.437717	562.314518	11.191424
10.721953	548.192151	11.196442
10.569152	558.188345	11.201459
10.267714	564.266279	11.206477
10.634523	551.399591	11.211495
10.206714	564.569394	11.216512
10.262926	550.009389	11.221530
10.232080	547.221407	11.226547
10.067163	555.815182	11.231565
10.533561	550.973782	11.236583
9.948002	559.226372	11.241600
9.993271	551.812734	11.246618
10.015554	557.477033	11.251635
10.494176	566.421257	11.256653
10.462656	575.022543	11.261671
10.297461	574.773910	11.266688
10.703689	575.562355	11.271706
10.629354	583.921048	11.276723
10.272037	584.699740	11.281741
10.472100	588.755152	11.286759
10.705328	585.651237	11.291776
10.804823	582.145402	11.296794
10.629787	575.943374	11.301811
10.786161	575.739030	11.306829
10.531714	571.357702	11.311847
10.441955	581.725878	11.316864
10.689590	575.653284	11.321882
10.417706	580.726215	11.326899
10.256203	587.833103	11.331917
10.654344	578.950381	11.336935
10.864975	587.504265	11.341952
10.864984	569.999248	11.346970
10.728832	581.087897	11.351987
10.815138	575.977843	11.357005
10.687333	580.624261	11.362023
10.702850	581.022648	11.367040
10.928839	580.861045	11.372058
10.656160	580.474620	11.377075
10.584695	577.538364	11.382093
10.569017	581.154212	11.387111
10.437424	578.852220	11.392128
10.429489	573.820048	11.397146
10.683457	581.357293	11.402163
10.252701	583.116313	11.407181
10.261929	578.788343	11.412199
10.956259	599.135298	11.417216
10.906931	601.910675	11.422234
11.106166	598.651139	11.427251
10.780640	592.879779	11.432269
10.903610	584.933251	11.437287
10.417787	587.029099	11.442304
10.904643	593.608376	11.447322
11.222017	607.627121	11.452339
10.816723	601.824075	11.457357
10.885381	585.870395	11.462375
10.861075	590.721503	11.467392
10.751229	603.241920	11.472410
11.119433	592.928004	11.477427
10.990545	601.449885	11.482445
10.994539	602.250862	11.487463
10.887460	599.623137	11.492480
10.694956	601.016628	11.497498
11.043523	615.024181	11.502515
10.804407	610.952862	11.507533
11.106783	605.622755	11.512551
11.073812	606.230710	11.517568
11.272039	599.648302	11.522586
11.105304	607.390328	11.527603
10.821586	611.136540	11.532621
11.270518	605.344818	11.537639
11.051440	607.976381	11.542656
11.294234	608.171903	11.547674
11.203068	601.060486	11.552691
10.850578	597.735918	11.557709
11.279716	596.071895	11.562727
11.149541	596.486798	11.567744
11.294543	600.228952	11.572762
11.200374	588.229719	11.577779
10.740176	575.603041	11.582797
11.198815	589.912060	11.587815
11.017008	608.575420	11.592832
11.207055	608.952774	11.597850
11.605606	604.806793	11.602867
11.053872	602.012054	11.607885
11.354505	589.275627	11.612903
11.387366	592.366325	11.617920
11.168272	584.564910	11.622938
11.180265	575.988841	11.627955
11.127547	584.902718	11.632973
11.501723	585.929713	11.637991
11.074752	592.507003	11.643008
11.319354	600.405481	11.648026
11.346732	596.093598	11.653043
11.116326	604.079126	11.658061
11.318662	604.871117	11.663079
11.376472	595.659861	11.668096
11.366821	601.748894	11.673114
11.584403	602.809892	11.678131
11.230457	610.726418	11.683149
11.706026	601.219333	11.688167
10.873781	597.222015	11.693184
11.188453	600.836600	11.698202
11.179463	603.040774	11.703219
11.313103	602.164657	11.708237
11.566999	601.515847	11.713255
11.512907	604.847388	11.718272
11.454939	608.454089	11.723290
11.473810	606.201101	11.728307
11.284113	601.124817	11.733325
11.592238	599.252539	11.738343
11.477882	599.216844	11.743360
11.409592	600.824401	11.748378
11.425492	597.678795	11.753395
11.269193	605.270864	11.758413
11.664405	600.326997	11.763431
11.475315	608.561671	11.768448
11.537029	607.990310	11.773466
11.386734	607.632045	11.778483
11.300087	605.581781	11.783501
11.357006	612.035924	11.788519
11.330550	613.712666	11.793536
11.381476	606.948209	11.798554
11.238481	601.602679	11.803571
11.431580	625.568975	11.808589
11.608516	627.390574	11.813607
11.947815	633.876221	11.818624
11.652657	626.108796	11.823642
11.859946	627.890925	11.828659
11.537805	618.979028	11.833677
11.413567	628.453237	11.838695
11.902706	635.171026	11.843712
11.859234	637.339582	11.848730
11.642576	631.286066	11.853747
11.380962	636.322690	11.858765
11.877627	632.473752	11.863783
12.026224	627.530647	11.868800
11.907289	637.720392	11.873818
11.787728	631.433915	11.878835
11.833750	625.932530	11.883853
11.867719	612.922290	11.888871
11.708333	615.579215	11.893888
11.598592	623.829866	11.898906
11.877536	629.908405	11.903923
11.822035	635.843689	11.908941
12.039575	629.939892	11.913959
12.240321	625.155874	11.918976
11.523345	622.169273	11.923994
11.793605	614.215433	11.929011
11.599463	625.076512	11.934029
11.676621	624.805685	11.939047
12.004855	625.439097	11.944064
11.833299	624.238415	11.949082
11.996756	621.618791	11.954099
11.748534	632.125433	11.959117
11.963261	628.642560	11.964135
11.867108	634.495851	11.969152
11.786570	635.606717	11.974170
12.260260	628.151169	11.979187
12.292036	624.441343	11.984205
11.868998	625.710012	11.989223
11.925327	621.384119	11.994240
11.741711	627.001805	11.999258
11.829134	623.289573	12.004275
11.797380	623.171508	12.009293
11.958709	624.165583	12.014311
12.018169	630.666672	12.019328
11.935311	628.514827	12.024346
12.052515	632.741021	12.029363
11.696994	651.283321	12.034381
12.192009	640.482454	12.039399
12.500249	656.112116	12.044416
12.100302	651.785123	12.049434
12.276479	644.231016	12.054451
12.034941	649.273966	12.059469
11.928417	648.097806	12.064487
12.340593	653.019397	12.069504
11.712111	662.518982	12.074522
11.860289	658.200780	12.079539
11.586937	654.671299	12.084557
11.843672	657.531273	12.089575
12.154727	652.363894	12.094592
12.053096	653.579050	12.099610
12.100573	653.284471	12.104627
12.355077	661.036259	12.109645
12.053962	675.221391	12.114663
12.668510	680.837113	12.119680
12.283368	669.542974	12.124698
12.466862	657.181456	12.129715
12.288655	656.038618	12.134733
12.400162	654.784116	12.139751
12.670635	654.309431	12.144768
12.582245	660.016349	12.149786
12.765449	653.789722	12.154803
12.461703	648.882772	12.159821
12.648943	657.654947	12.164839
12.446592	648.405532	12.169856
12.514425	645.851380	12.174874
12.683819	649.728577	12.179891
12.372388	659.980053	12.184909
12.356833	660.787251	12.189927
12.632668	655.783178	12.194944
12.636120	657.666675	12.199962
12.599085	653.371182	12.204979
12.429381	656.581991	12.209997
12.659575	656.987770	12.215015
12.748077	657.100171	12.220032
12.499547	659.035772	12.225050
12.745428	658.186247	12.230067
12.874116	652.690837	12.235085
12.452531	652.974676	12.240103
12.807415	647.090379	12.245120
11.992418	652.163219	12.250138
12.579385	643.515965	12.255155
12.866485	651.442522	12.260173
12.536111	644.251802	12.265191
12.640941	641.612960	12.270208
12.997640	645.558638	12.275226
13.072950	652.830418	12.280243
12.552429	655.742746	12.285261
12.660627	661.747064	12.290279
12.894607	649.882566	12.295296
12.583922	655.649558	12.300314
12.840123	648.259635	12.305331
12.716058	648.414808	12.310349
12.930898	659.022481	12.315367
12.911266	659.224407	12.320384
12.979206	654.959803	12.325402
13.087265	652.058523	12.330419
12.886382	643.717745	12.335437
12.983734	647.704058	12.340455
12.973113	634.798617	12.345472
12.695418	631.620112	12.350490
12.356621	625.257534	12.355507
12.872087	644.688989	12.360525
12.866201	650.938394	12.365543
13.145539	642.134214	12.370560
12.735922	647.957729	12.375578
12.954769	648.415778	12.380595
13.005235	649.834320	12.385613
13.040828	649.813000	12.390631
13.170999	645.623854	12.395648
13.012575	643.789957	12.400666
12.790671	651.430194	12.405683
12.857097	656.601616	12.410701
12.711106	658.742057	12.415719
12.835314	660.710775	12.420736
12.655218	660.994647	12.425754
12.987973	652.163159	12.430771
12.794140	649.160858	12.435789
12.607982	650.887872	12.440807
12.604371	653.012315	12.445824
12.919465	674.589570	12.450842
12.727970	669.261086	12.455859
13.335725	677.572912	12.460877
12.677605	685.246796	12.465895
13.109231	681.177666	12.470912
12.890763	676.178451	12.475930
12.871818	683.979405	12.480947
13.191046	679.984690	12.485965
13.126631	678.969188	12.490983
13.263989	667.454330	12.496000
13.266960	678.631694	12.501018
13.128842	678.908989	12.506035
13.017047	679.516673	12.511053
13.057655	680.573847	12.516071
13.459763	670.816304	12.521088
13.169412	682.696032	12.526106
12.931745	671.662807	12.531123
12.693641	677.096543	12.536141
13.084493	699.678122	12.541159
13.544692	701.906625	12.546176
13.650370	697.146950	12.551194
13.504926	701.395378	12.556211
13.650904	702.120464	12.561229
13.568516	697.103079	12.566247
13.324347	673.867434	12.571264
13.293827	685.592845	12.576282
13.370923	686.940946	12.581299
13.661703	699.900431	12.586317
13.310499	686.944173	12.591335
13.342721	684.051615	12.596352
13.777850	699.894963	12.601370
13.414753	690.004840	12.606387
13.499397	687.580592	12.611405
13.561362	701.888736	12.616423
13.460067	684.273248	12.621440
13.634850	689.336185	12.626458
13.427188	686.007843	12.631475
13.678894	693.589671	12.636493
13.654832	692.826620	12.641511
13.430263	682.084825	12.646528
13.730161	692.401481	12.651546
13.278882	698.023258	12.656563
13.784400	701.898294	12.661581
13.613977	704.623234	12.666599
13.718930	698.535084	12.671616
13.611229	705.908143	12.676634
13.718574	694.394815	12.681651
13.817404	703.543781	12.686669
13.914498	700.357034	12.691687
13.585652	697.158130	12.696704
13.778333	705.090037	12.701722
13.860260	711.729646	12.706739
13.620894	701.315203	12.711757
13.826138	707.405317	12.716775
13.836781	697.257817	12.721792
13.826280	702.056300	12.726810
14.045022	703.366430	12.731827
14.062213	684.394321	12.736845
13.850490	682.565615	12.741863
13.518508	673.674167	12.746880
13.523378	678.703763	12.751898
13.429840	694.920272	12.756915
13.454656	701.925429	12.761933
13.814516	712.582996	12.766951
13.918608	703.304473	12.771968
13.475227	702.102194	12.776986
13.433652	712.226212	12.782003
14.036739	704.030838	12.787021
13.833509	711.702888	12.792039
14.006328	704.461707	12.797056
13.979501	706.236345	12.802074
13.784318	700.378255	12.807091
13.894141	705.271495	12.812109
14.073802	720.233398	12.817127
14.297234	717.717972	12.822144
14.204876	712.560133	12.827162
13.774253	705.066361	12.832179
13.889025	703.479987	12.837197
14.124042	726.284831	12.842215
14.543869	728.090475	12.847232
14.448865	722.456523	12.852250
14.054797	715.761746	12.857267
14.007369	712.171609	12.862285
14.013495	708.923375	12.867303
14.011568	707.680331	12.872320
14.133812	705.247032	12.877338
13.949482	718.056910	12.882355
14.731042	726.745469	12.887373
14.496635	716.664755	12.892391
13.962691	706.681470	12.897408
13.959301	706.016165	12.902426
14.048665	723.415866	12.907443
14.301600	720.425604	12.912461
14.519132	723.515794	12.917479
14.238712	723.007502	12.922496
14.317072	729.518289	12.927514
14.473387	728.155776	12.932531
14.912741	721.456648	12.937549
14.408287	716.363376	12.942567
14.371287	699.820236	12.947584
14.486117	698.117088	12.952602
13.990343	702.795944	12.957619
14.472835	703.809131	12.962637
14.132994	726.227520	12.967655
14.105213	720.939641	12.972672
14.381789	713.603304	12.977690
14.357656	723.450042	12.982707
14.722877	714.203183	12.987725
14.535053	720.326484	12.992743
14.411372	724.410562	12.997760
14.885788	722.780459	13.002778
14.770400	721.813966	13.007795
14.691428	721.498173	13.012813
14.429805	727.399511	13.017831
14.745947	722.105082	13.022848
14.142764	724.995660	13.027866
14.266174	726.854058	13.032883
14.334344	722.983875	13.037901
14.558194	733.732192	13.042919
14.309171	731.735756	13.047936
14.283797	717.576560	13.052954
14.405396	732.882084	13.057971
14.686173	724.835030	13.062989
14.643676	730.821957	13.068007
14.588710	729.277953	13.073024
14.753800	733.222114	13.078042
14.981647	747.084584	13.083059
15.129564	740.730912	13.088077
14.720976	729.109050	13.093095
14.368354	727.744227	13.098112
14.484545	730.156021	13.103130
14.916065	748.095427	13.108147
14.778800	743.032978	13.113165
15.049755	751.426010	13.118183
15.087862	750.009433	13.123200
14.684486	752.742477	13.128218
14.574256	750.004771	13.133235
14.667025	750.769754	13.138253
14.704277	754.692924	13.143271
15.093567	751.353089	13.148288
14.932200	754.976020	13.153306
15.042640	756.287344	13.158323
15.263365	746.798021	13.163341
15.223571	761.049573	13.168359
15.015860	740.512652	13.173376
14.903978	745.778310	13.178394
14.774933	744.356365	13.183411
15.086615	742.429866	13.188429
15.015200	750.497846	13.193447
14.835317	755.266077	13.198464
15.081863	743.693037	13.203482
14.642261	746.463314	13.208499
14.978377	739.887652	13.213517
14.912577	749.971306	13.218535
14.907267	751.221871	13.223552
15.085367	746.450836	13.228570
14.776381	758.639646	13.233587
15.201675	751.434626	13.238605
15.245749	754.959096	13.243623
15.097465	766.166525	13.248640
15.463864	768.450759	13.253658
15.422754	771.878126	13.258675
15.437496	755.027027	13.263693
15.067866	747.088180	13.268711
14.849475	759.019799	13.273728
15.641762	763.777724	13.278746
15.101978	770.811411	13.283763
15.222860	779.221659	13.288781
15.610629	779.994071	13.293799
15.142324	776.296295	13.298816
15.507234	772.587892	13.303834
15.188621	778.608629	13.308851
15.449194	767.822327	13.313869
15.689166	774.740154	13.318887
15.295064	779.216908	13.323904
15.493414	778.377981	13.328922
15.725761	781.746726	13.333939
15.686211	766.245339	13.338957
15.478894	764.144535	13.343975
15.065653	761.612093	13.348992
15.540776	761.348338	13.354010
15.348838	767.579598	13.359027
15.809785	767.043509	13.364045
15.502075	765.570661	13.369063
15.758413	772.653180	13.374080
15.672388	772.985431	13.379098
15.653713	775.973783	13.384115
15.742059	771.699642	13.389133
15.728277	775.583475	13.394151
15.793361	770.625014	13.399168
15.437727	759.900551	13.404186
15.388268	774.683803	13.409203
15.879618	775.503102	13.414221
15.793713	782.004932	13.419239
15.844900	777.711365	13.424256
15.695595	765.111581	13.429274
15.783961	770.838176	13.434291
15.665559	769.064267	13.439309
15.693671	767.128547	13.444327
15.727102	771.004983	13.449344
15.805711	767.833743	13.454362
15.632575	774.058904	13.459379
15.459869	773.656810	13.464397
15.803564	769.655086	13.469415
15.622385	774.663366	13.474432
15.757475	760.854535	13.479450
15.607370	779.333225	13.484467
15.641058	771.160762	13.489485
15.675522	765.705327	13.494503
15.678552	775.270127	13.499520
16.147789	781.653419	13.504538
16.002405	789.622552	13.509555
16.148649	798.577946	13.514573
16.418947	786.287945	13.519591
15.820169	774.803149	13.524608
15.981289	771.095118	13.529626
16.161117	775.687075	13.534643
15.899648	771.448808	13.539661
16.308053	772.180117	13.544679
16.018675	777.833357	13.549696
15.982927	775.020860	13.554714
16.312547	781.441806	13.559731
16.260077	775.116363	13.564749
16.277087	765.053034	13.569767
16.136581	777.363782	13.574784
16.090061	755.936897	13.579802
16.365401	764.748971	13.584819
16.256775	764.996400	13.589837
16.281353	759.877030	13.594855
16.128607	763.558572	13.599872
16.391396	765.003817	13.604890
16.412680	769.248228	13.609907
16.357714	765.779182	13.614925
16.198678	769.010431	13.619943
16.377863	758.653452	13.624960
16.472340	764.760940	13.629978
16.308276	768.008756	13.634995
16.213262	773.928186	13.640013
16.418162	773.662589	13.645031
16.427487	791.999548	13.650048
16.607332	785.662949	13.655066
16.518822	792.673275	13.660083
16.227901	784.961921	13.665101
16.821731	787.608155	13.670119
16.348680	789.124512	13.675136
16.661375	781.760397	13.680154
16.712045	773.373833	13.685171
16.508307	766.463024	13.690189
16.382905	770.354878	13.695207
16.429319	782.229244	13.700224
16.633306	786.568110	13.705242
16.698327	787.716139	13.710259
16.472407	785.009177	13.715277
16.701117	786.469230	13.720295
16.351249	789.629397	13.725312
16.466347	789.743943	13.730330
16.746296	792.758093	13.735347
16.528846	787.635611	13.740365
16.606039	789.649580	13.745383
16.547884	793.625577	13.750400
16.536678	788.511806	13.755418
16.297103	788.975412	13.760435
16.592255	788.926047	13.765453
16.580811	780.656510	13.770471
16.375589	792.949006	13.775488
16.873718	804.354980	13.780506
16.840230	814.111716	13.785523
16.886492	824.367203	13.790541
17.382485	823.386964	13.795559
16.960652	809.406577	13.800576
16.818885	797.537737	13.805594
16.916854	793.457743	13.810611
16.721266	792.248192	13.815629
16.856771	797.049070	13.820647
16.711214	813.908154	13.825664
16.841177	812.489803	13.830682
17.049194	818.169265	13.835699
16.911266	819.128187	13.840717
17.342936	817.340672	13.845735
17.183151	819.716822	13.850752
17.346098	811.290559	13.855770
17.072632	799.215134	13.860787
17.192041	808.436669	13.865805
16.933152	802.241389	13.870823
16.841411	806.314169	13.875840
17.165558	807.235407	13.880858
17.404005	808.662379	13.885875
16.680679	819.404516	13.890893
17.160499	813.172386	13.895911
16.823138	815.667877	13.900928
17.324775	813.225614	13.905946
17.048752	807.758853	13.910963
16.948839	812.154807	13.915981
17.091918	799.884729	13.920999
17.273787	805.309508	13.926016
17.347854	807.592212	13.931034
17.358671	809.913229	13.936051
17.084519	813.522285	13.941069
17.630955	805.433571	13.946087
17.249860	808.668061	13.951104
17.288724	803.600090	13.956122
17.272162	808.557341	13.961139
17.292464	809.425199	13.966157
17.310079	815.667824	13.971175
17.313119	824.143894	13.976192
17.901062	823.190274	13.981210
17.658159	815.995248	13.986227
17.591890	811.634869	13.991245
17.626501	805.459874	13.996263
17.393951	809.602054	14.001280
17.418396	803.037332	14.006298
17.733965	816.845086	14.011315
17.637607	816.692961	14.016333
17.581266	810.633201	14.021351
17.274680	823.995641	14.026368
17.913785	824.536171	14.031386
18.058328	821.944729	14.036403
17.510543	818.262552	14.041421
17.283806	810.351782	14.046439
17.449121	822.182299	14.051456
17.727645	822.280707	14.056474
17.830087	823.356603	14.061491
17.717192	824.235864	14.066509
18.032341	823.075676	14.071527
17.947999	829.012388	14.076544
18.011431	837.185511	14.081562
18.221697	828.754981	14.086579
17.879003	829.310485	14.091597
17.902694	809.516713	14.096615
17.756322	819.672991	14.101632
17.863200	826.188813	14.106650
18.063885	818.334147	14.111667
17.955874	824.826833	14.116685
17.865850	816.919885	14.121703
18.097839	826.780200	14.126720
18.020261	829.228679	14.131738
18.028518	817.658212	14.136755
17.936821	824.419741	14.141773
18.081795	819.896875	14.146791
17.943419	828.373013	14.151808
18.026096	824.544717	14.156826
18.072180	828.109913	14.161843
18.088455	838.313302	14.166861
18.525819	825.997097	14.171879
18.322047	820.430649	14.176896
17.951597	809.421298	14.181914
17.975441	807.050740	14.186931
17.931306	820.798091	14.191949
18.359969	818.834322	14.196967
18.096630	826.020376	14.201984
18.192810	824.452683	14.207002
18.185469	823.784837	14.212019
18.130555	816.153256	14.217037
18.383768	811.976350	14.222055
18.196816	826.175272	14.227072
18.149805	819.826868	14.232090
18.408523	821.515753	14.237107
18.194878	831.423801	14.242125
18.645217	824.132777	14.247143
18.584336	825.016512	14.252160
18.447591	822.753165	14.257178
18.430008	818.858528	14.262195
18.260415	829.100501	14.267213
18.581684	829.586688	14.272231
18.592022	833.507781	14.277248
18.322753	825.849821	14.282266
18.104567	824.760573	14.287283
18.432373	828.407861	14.292301
18.534116	824.472436	14.297319
18.878413	820.132934	14.302336
18.650326	818.764370	14.307354
18.519673	827.816812	14.312371
18.424766	821.983997	14.317389
18.718299	819.198797	14.322407
18.654983	823.456477	14.327424
18.195045	830.140004	14.332442
18.549690	830.097097	14.337459
18.881014	852.344214	14.342477
18.886888	835.286144	14.347495
18.819003	833.942972	14.352512
18.207163	829.980494	14.357530
18.748930	836.791100	14.362547
18.595041	842.113861	14.367565
18.592227	855.463443	14.372583
19.138916	836.196772	14.377600
19.052091	850.730320	14.382618
19.180466	846.080659	14.387635
19.000111	849.649779	14.392653
19.072314	837.504390	14.397671
18.685449	845.009609	14.402688
18.769487	846.577541	14.407706
19.031578	852.844991	14.412723
18.702815	851.810936	14.417741
19.000302	845.604208	14.422759
19.266287	837.461590	14.427776
19.029582	842.005217	14.432794
19.321938	841.789033	14.437811
19.038843	846.399890	14.442829
18.766416	836.940448	14.447847
19.042677	836.442762	14.452864
18.816425	846.570546	14.457882
19.170615	836.545866	14.462899
18.738602	848.043954	14.467917
19.058453	841.754827	14.472935
19.063361	836.029445	14.477952
18.823791	842.672138	14.482970
19.225777	855.399717	14.487987
19.220980	864.811156	14.493005
19.308221	876.208971	14.498023
19.757073	861.429402	14.503040
19.191605	861.701072	14.508058
19.326985	853.298043	14.513075
19.534037	856.424612	14.518093
19.372923	847.143385	14.523111
19.361009	844.513337	14.528128
19.251192	852.480082	14.533146
19.272637	852.129617	14.538163
19.486817	855.315030	14.543181
19.785410	856.082483	14.548199
19.804548	858.853485	14.553216
19.391538	847.509950	14.558234
19.343688	840.060290	14.563251
19.366479	856.886726	14.568269
19.662037	863.511855	14.573287
20.102882	858.125264	14.578304
19.494748	848.453327	14.583322
19.514135	835.984853	14.588339
19.207091	841.924903	14.593357
19.672592	849.817285	14.598375
19.707559	854.466673	14.603392
20.060469	865.589326	14.608410
20.000046	855.515987	14.613427
19.445428	853.311796	14.618445
19.488276	861.639635	14.623463
19.698616	863.531765	14.628480
19.783947	853.542888	14.633498
19.916976	862.017545	14.638515
19.498180	858.188917	14.643533
19.504083	860.510710	14.648551
19.899604	855.197494	14.653568
20.230592	852.699912	14.658586
20.068333	857.670537	14.663603
19.871860	859.721081	14.668621
19.829146	860.586192	14.673639
20.095542	857.177230	14.678656
19.810003	860.267369	14.683674
20.149316	857.355070	14.688691
19.805650	864.547414	14.693709
20.047943	858.289368	14.698727
20.234053	856.732828	14.703744
19.737323	861.370849	14.708762
19.782631	855.591794	14.713779
19.521425	867.908892	14.718797
19.967100	868.669081	14.723815
20.279383	875.597708	14.728832
20.218077	883.739904	14.733850
20.350544	879.026476	14.738867
20.430096	875.255464	14.743885
20.399244	867.563287	14.748903
20.489808	858.217375	14.753920
20.115526	858.067769	14.758938
19.876389	854.015332	14.763955
20.131299	879.988855	14.768973
20.197902	881.180823	14.773991
20.107922	874.252149	14.779008
20.487659	892.177723	14.784026
20.519793	879.208601	14.789043
20.654173	885.196269	14.794061
20.490253	880.885887	14.799079
20.759451	881.487533	14.804096
20.739790	881.320235	14.809114
20.205987	868.670167	14.814131
20.143526	864.381762	14.819149
20.313983	867.643455	14.824167
20.196281	874.715192	14.829184
20.019502	871.770142	14.834202
20.196151	865.850584	14.839219
20.291739	863.118482	14.844237
20.106776	877.822065	14.849255
20.489755	891.613004	14.854272
20.610908	899.915968	14.859290
20.717314	906.738009	14.864307
20.824857	902.101064	14.869325
20.647585	908.042895	14.874343
21.301852	899.858348	14.879360
20.921673	903.168451	14.884378
20.917119	903.762496	14.889395
20.958983	888.851010	14.894413
20.581001	891.400213	14.899431
20.961926	890.930308	14.904448
20.641515	898.819616	14.909466
20.841255	901.833728	14.914483
20.906438	900.311911	14.919501
21.038732	902.569725	14.924519
21.023802	902.979202	14.929536
21.179499	910.554075	14.934554
20.974320	910.788231	14.939571
20.925536	902.855849	14.944589
21.026094	907.703259	14.949607
21.334522	902.050222	14.954624
20.959159	900.856207	14.959642
21.306665	902.496474	14.964659
21.550311	891.400323	14.969677
20.881395	883.868071	14.974695
20.993375	880.183496	14.979712
20.860886	889.700162	14.984730
21.106085	899.634187	14.989747
21.081435	900.900416	14.994765
21.147419	897.989909	14.999783
20.932155	904.934932	15.004800
21.096357	912.375929	15.009818
21.082937	899.300320	15.014835
21.478885	905.527881	15.019853
21.034584	906.130865	15.024871
21.507802	894.537992	15.029888
20.966580	903.771565	15.034906
21.209014	902.790024	15.039923
21.299971	898.212485	15.044941
21.469216	902.831379	15.049959
21.328509	906.779310	15.054976
21.495151	916.817172	15.059994
21.647321	919.270691	15.065011
22.167784	920.214826	15.070029
21.319966	911.381988	15.075047
21.431099	904.478596	15.080064
21.252816	908.385077	15.085082
21.591929	915.489399	15.090099
21.666244	925.185123	15.095117
21.574960	921.718580	15.100135
21.953072	918.118533	15.105152
21.736087	918.250397	15.110170
21.657310	924.375618	15.115187
21.860907	918.824208	15.120205
21.771566	921.296632	15.125223
22.014195	907.748551	15.130240
21.381265	909.204760	15.135258
21.505526	914.070549	15.140275
21.778449	912.137482	15.145293
22.015265	918.762368	15.150311
22.107757	912.824422	15.155328
21.944020	923.311685	15.160346
21.924859	914.667751	15.165363
22.140174	909.392221	15.170381
21.878052	913.065684	15.175399
21.995577	905.981408	15.180416
21.722219	914.396684	15.185434
22.237837	916.916336	15.190451
22.345773	914.696692	15.195469
22.184815	918.344839	15.200487
22.339253	914.767214	15.205504
21.880998	899.694234	15.210522
21.905006	909.814400	15.215539
21.940284	901.881471	15.220557
21.871215	913.370073	15.225575
22.186797	903.026354	15.230592
22.521912	917.705289	15.235610
22.377826	908.329844	15.240627
22.359485	908.298039	15.245645
22.347842	911.320026	15.250663
22.373879	900.933311	15.255680
22.372374	915.081157	15.260698
22.051354	911.795780	15.265715
22.469392	907.813935	15.270733
22.231071	911.736135	15.275751
22.453820	900.352917	15.280768
22.212593	909.233375	15.285786
22.064267	908.978937	15.290803
22.455073	903.278279	15.295821
22.158380	904.530326	15.300839
22.304405	906.028592	15.305856
22.501235	904.612380	15.310874
22.252975	907.049742	15.315891
22.536537	907.983656	15.320909
22.667642	928.854740	15.325927
22.815664	929.992930	15.330944
22.463934	927.668578	15.335962
22.526042	932.297954	15.340979
22.819177	939.292724	15.345997
22.542888	941.605093	15.351015
22.645647	936.924707	15.356032
22.799785	940.356230	15.361050
22.935069	938.558335	15.366067
23.227856	925.314810	15.371085
22.937491	927.793485	15.376103
22.891591	922.637774	15.381120
22.935504	930.760349	15.386138
22.879887	928.162383	15.391155
23.303621	917.707036	15.396173
22.848895	920.138878	15.401191
22.685309	915.582281	15.406208
22.717409	915.712988	15.411226
22.992778	924.061229	15.416243
22.978899	925.786523	15.421261
23.170463	933.194839	15.426279
23.436187	927.722056	15.431296
23.373302	918.084572	15.436314
23.180719	918.755415	15.441331
23.197465	909.859702	15.446349
23.067002	916.176056	15.451367
23.068285	915.349064	15.456384
23.143409	933.682171	15.461402
23.171956	932.374376	15.466419
23.652912	929.241055	15.471437
23.124803	933.599986	15.476455
23.173442	923.083484	15.481472
23.308871	920.783792	15.486490
23.431151	926.621890	15.491507
23.365313	925.881154	15.496525
23.498072	922.938090	15.501543
23.597570	920.293730	15.506560
23.662262	916.764880	15.511578
23.381712	905.593060	15.516595
23.232376	898.812532	15.521613
23.273772	915.386798	15.526631
23.551979	916.564551	15.531648
23.361727	930.303321	15.536666
23.294372	924.478779	15.541683
23.469944	922.643016	15.546701
22.910672	935.496015	15.551719
23.208433	930.889221	15.556736
23.611339	922.141283	15.561754
23.562237	931.935244	15.566771
23.329390	933.881040	15.571789
23.728652	945.239480	15.576807
23.768658	949.212754	15.581824
23.861395	953.253508	15.586842
24.001413	943.057196	15.591859
24.112356	940.168041	15.596877
23.799494	926.754316	15.601895
23.582583	915.411572	15.606912
24.154554	930.204886	15.611930
24.137978	936.257249	15.616947
23.917934	921.352056	15.621965
23.586069	922.019475	15.626983
23.582369	938.635543	15.632000
23.702771	933.917680	15.637018
23.770236	942.147025	15.642035
23.983072	940.125539	15.647053
23.794677	954.637216	15.652071
24.069778	940.023662	15.657088
24.494630	942.077852	15.662106
24.082541	955.362245	15.667123
24.398683	945.400271	15.672141
23.997544	953.447419	15.677159
24.039541	937.630146	15.682176
24.171914	944.432353	15.687194
23.978726	952.721477	15.692211
24.065322	942.129588	15.697229
24.134264	950.822613	15.702247
23.869507	953.780122	15.707264
24.168084	958.438728	15.712282
24.248690	972.431742	15.717299
24.358011	966.162934	15.722317
25.005446	978.290406	15.727335
24.350920	971.219769	15.732352
24.504414	966.970089	15.737370
24.367910	978.958453	15.742387
24.630446	968.970150	15.747405
24.716480	969.755133	15.752423
24.821558	977.315875	15.757440
24.738157	969.186914	15.762458
24.747392	967.837960	15.767475
24.475692	963.317224	15.772493
24.480283	969.546164	15.777511
24.854695	962.036605	15.782528
24.917056	960.606743	15.787546
24.873706	963.381240	15.792563
24.936600	964.731588	15.797581
25.297207	958.985150	15.802599
25.107489	950.503622	15.807616
24.904610	943.138169	15.812634
24.424107	940.505785	15.817651
24.590186	940.568163	15.822669
24.459555	948.071148	15.827687
24.586927	959.749909	15.832704
24.679460	954.588279	15.837722
24.459390	962.805879	15.842739
24.535102	960.736446	15.847757
24.756267	965.984702	15.852775
24.251017	968.411843	15.857792
24.782644	969.688750	15.862810
24.900933	985.859711	15.867827
24.880815	991.306725	15.872845
25.280605	985.380569	15.877863
25.018056	989.259244	15.882880
25.107395	994.543941	15.887898
25.096984	991.683259	15.892915
25.390959	985.470721	15.897933
25.225418	980.974373	15.902951
25.150233	988.030026	15.907968
25.604201	987.400351	15.912986
25.164366	991.227907	15.918003
25.130934	982.712409	15.923021
25.527980	979.071513	15.928039
25.630063	982.580629	15.933056
25.439178	979.852368	15.938074
25.604805	981.461179	15.943091
25.568863	984.799413	15.948109
25.500009	986.457586	15.953127
25.251260	991.148307	15.958144
25.734352	976.918706	15.963162
25.259969	987.890185	15.968179
25.356330	987.035669	15.973197
25.449001	997.833101	15.978215
25.590230	1007.007139	15.983232
25.893414	1005.662620	15.988250
26.209322	1016.043230	15.993267
26.097644	996.746993	15.998285
26.115960	988.557904	16.003303
25.923238	989.288732	16.008320
25.902081	979.935014	16.013338
25.666406	984.967671	16.018355
25.692301	982.341146	16.023373
25.735338	989.012199	16.028391
25.834218	995.295803	16.033408
25.860644	979.433596	16.038426
25.946826	988.041886	16.043443
25.867862	995.391627	16.048461
25.861366	988.547658	16.053479
26.065348	1007.015288	16.058496
26.417223	1006.344803	16.063514
26.348034	1003.332380	16.068531
26.242634	980.453294	16.073549
25.928334	987.852528	16.078567
25.949979	985.182486	16.083584
26.194798	998.240909	16.088602
26.537811	1002.905189	16.093619
26.364866	996.980400	16.098637
26.215415	1002.387721	16.103655
26.245172	1003.146809	16.108672
26.404756	1008.297427	16.113690
26.192213	1015.983690	16.118707
25.991926	1007.917206	16.123725
26.158739	1001.386910	16.128743
26.232797	1012.026319	16.133760
26.311616	1004.171731	16.138778
26.319314	1008.673951	16.143795
26.146104	1007.978437	16.148813
26.653587	1005.213336	16.153831
26.291895	1004.427431	16.158848
26.609580	1000.360303	16.163866
26.591029	1009.720325	16.168883
26.409290	1005.147613	16.173901
26.601100	1004.379129	16.178919
26.514902	1004.834488	16.183936
26.928814	1012.116480	16.188954
26.668297	1010.857125	16.193971
26.679206	1007.870022	16.198989
26.760869	1011.417057	16.204007
26.664481	1019.435421	16.209024
26.993461	1025.036036	16.214042
26.825486	1027.542887	16.219059
26.722082	1029.509438	16.224077
26.954229	1016.003944	16.229095
27.010109	1032.023776	16.234112
27.408950	1023.945466	16.239130
27.049322	1019.883467	16.244147
26.718977	1006.604967	16.249165
27.086179	1016.513631	16.254183
27.196611	1030.246394	16.259200
27.321318	1024.827234	16.264218
27.049516	1013.452000	16.269235
26.733519	1012.065636	16.274253
27.261037	1023.284109	16.279271
26.815541	1024.540543	16.284288
27.233233	1014.436386	16.289306
27.390790	1022.787354	16.294323
27.341161	1025.300909	16.299341
27.625483	1025.155410	16.304359
27.122827	1021.526080	16.309376
27.395930	1022.240730	16.314394
27.561887	1018.920059	16.319411
27.544131	1021.349724	16.324429
27.469018	1017.151628	16.329447
27.451609	1020.382823	16.334464
27.236849	1026.305319	16.339482
27.255243	1020.524116	16.344499
27.015859	1023.143141	16.349517
27.398951	1014.732784	16.354535
27.242811	1020.485145	16.359552
27.656542	1022.790400	16.364570
27.552999	1014.995937	16.369587
27.561597	1021.969048	16.374605
27.667074	1033.007495	16.379623
27.862080	1049.564130	16.384640
28.070832	1037.132119	16.389658
27.573804	1024.807541	16.394675
27.461859	1040.011064	16.399693
27.816323	1036.733440	16.404711
28.036392	1038.412622	16.409728
28.689570	1029.679070	16.414746
28.332564	1024.426904	16.419763
27.985452	1012.205080	16.424781
27.604409	1006.962997	16.429799
27.857967	1016.220427	16.434816
28.210594	1016.190461	16.439834
28.195605	1005.182099	16.444851
27.922616	1012.628520	16.449869
28.406076	1011.561872	16.454887
28.114820	1025.632126	16.459904
28.352503	1014.303300	16.464922
28.009271	1009.276202	16.469939
27.890971	1014.972139	16.474957
28.355211	1019.658455	16.479975
28.349698	1033.706037	16.484992
28.518523	1032.982178	16.490010
28.591782	1026.207752	16.495027
28.221114	1032.899458	16.500045
28.415260	1026.607871	16.505063
28.546672	1036.408320	16.510080
28.400437	1028.756242	16.515098
28.455634	1024.354689	16.520115
28.555948	1032.900825	16.525133
28.602053	1026.386277	16.530151
28.341905	1027.376983	16.535168
28.344051	1035.506150	16.540186
28.509715	1030.850599	16.545203
28.475410	1034.119158	16.550221
28.737854	1030.521432	16.555239
28.434351	1027.640392	16.560256
28.358759	1031.237316	16.565274
28.654265	1029.875063	16.570291
28.345268	1030.292747	16.575309
28.550892	1026.255794	16.580327
28.313918	1030.032639	16.585344
28.769475	1040.552331	16.590362
28.387099	1052.285774	16.595379
28.544899	1047.549398	16.600397
28.659468	1034.207480	16.605415
28.820787	1046.786709	16.610432
28.705154	1053.984427	16.615450
29.077908	1043.612735	16.620467
28.867792	1051.352282	16.625485
28.938566	1041.217256	16.630503
29.340705	1057.315406	16.635520
29.343272	1046.657724	16.640538
29.402644	1053.130579	16.645555
29.184723	1048.708694	16.650573
29.465858	1046.184183	16.655591
29.270218	1047.616069	16.660608
29.394762	1047.438799	16.665626
29.608420	1040.367810	16.670643
29.095868	1051.178048	16.675661
29.503431	1044.464847	16.680679
29.474795	1054.340876	16.685696
29.474380	1049.433626	16.690714
29.521219	1042.306721	16.695731
29.174553	1049.698428	16.700749
29.227495	1036.987867	16.705767
29.652381	1055.231585	16.710784
29.964657	1064.770179	16.715802
29.945169	1049.940755	16.720819
29.478759	1044.304931	16.725837
29.425025	1044.133503	16.730855
29.791188	1053.354374	16.735872
29.208986	1044.094838	16.740890
29.804851	1061.551214	16.745907
29.682626	1066.550339	16.750925
29.873905	1066.637172	16.755943
29.758669	1071.758282	16.760960
29.881462	1074.443648	16.765978
30.302494	1069.634465	16.770995
29.907424	1075.133941	16.776013
29.981697	1072.528225	16.781031
29.744804	1071.653334	16.786048
30.045931	1071.445241	16.791066
30.234528	1063.652323	16.796083
30.111609	1074.524606	16.801101
30.288414	1071.088616	16.806119
30.110362	1068.961099	16.811136
29.929587	1067.793389	16.816154
30.293665	1056.192265	16.821171
30.003116	1070.126741	16.826189
30.021317	1066.011845	16.831207
30.106607	1070.855380	16.836224
30.276238	1067.666670	16.841242
30.583097	1061.764517	16.846259
30.151386	1072.609439	16.851277
30.009729	1066.480906	16.856295
30.154700	1073.091838	16.861312
30.056026	1060.042092	16.866330
30.380912	1070.424483	16.871347
30.132933	1079.116731	16.876365
30.416332	1088.517849	16.881383
30.617316	1088.423278	16.886400
30.669935	1097.936300	16.891418
30.964557	1084.891188	16.896435
30.642986	1094.428121	16.901453
30.801771	1090.073439	16.906471
30.846310	1093.102433	16.911488
30.666171	1082.542785	16.916506
31.166088	1087.671662	16.921523
30.760308	1079.122937	16.926541
30.821044	1075.178102	16.931559
30.977677	1080.897258	16.936576
30.922436	1080.533558	16.941594
31.385879	1079.567874	16.946611
30.905246	1081.861783	16.951629
30.791262	1062.045120	16.956647
30.886433	1068.490280	16.961664
30.595266	1086.221361	16.966682
30.962642	1079.776379	16.971699
31.004091	1080.224364	16.976717
31.084870	1085.545145	16.981735
30.841300	1080.290968	16.986752
30.778024	1078.265390	16.991770
31.057020	1081.304986	16.996787
30.872531	1089.700109	17.001805
30.953548	1081.084580	17.006823
31.344791	1100.182541	17.011840
31.222685	1095.969699	17.016858
31.084177	1097.641951	17.021875
31.192864	1101.408836	17.026893
31.346582	1098.430901	17.031911
31.229590	1088.476749	17.036928
31.232894	1090.871564	17.041946
31.475606	1096.406821	17.046963
31.048327	1099.238337	17.051981
31.086559	1108.043550	17.056999
31.459420	1110.711832	17.062016
31.370495	1116.829241	17.067034
31.688897	1117.539953	17.072051
31.831683	1126.814797	17.077069
32.117480	1113.692150	17.082087
32.018411	1121.297562	17.087104
31.825605	1118.765244	17.092122
32.047835	1116.133185	17.097139
32.011780	1116.492327	17.102157
31.888859	1110.701676	17.107175
31.792954	1113.689562	17.112192
32.044153	1113.577655	17.117210
32.114570	1106.721591	17.122227
32.205010	1111.094106	17.127245
32.321988	1108.535344	17.132263
32.651256	1107.170952	17.137280
32.172549	1110.307178	17.142298
32.200340	1105.600624	17.147315
32.553114	1109.136760	17.152333
32.442956	1103.243124	17.157351
32.270684	1089.125584	17.162368
31.880289	1088.470406	17.167386
32.209212	1099.117273	17.172403
32.479877	1111.344894	17.177421
32.406903	1102.011855	17.182439
32.713984	1108.275502	17.187456
32.362960	1108.775512	17.192474
32.540710	1101.744840	17.197491
32.342762	1113.556726	17.202509
32.429290	1113.360165	17.207527
32.874514	1108.888014	17.212544
32.178896	1112.380124	17.217562
32.278623	1108.646927	17.222579
32.612593	1109.415162	17.227597
32.626967	1111.246502	17.232615
32.635624	1107.208833	17.237632
32.360899	1118.328994	17.242650
32.391370	1105.271604	17.247667
32.546521	1106.692716	17.252685
32.299452	1119.755712	17.257703
32.714152	1133.390388	17.262720
32.597523	1135.737727	17.267738
33.238851	1134.927211	17.272755
32.785191	1131.334363	17.277773
32.943022	1129.532917	17.282791
33.298149	1129.221687	17.287808
32.845565	1131.167218	17.292826
33.240602	1130.079704	17.297843
33.546999	1134.724508	17.302861
33.179528	1124.535020	17.307879
33.855382	1119.193583	17.312896
33.122821	1137.173755	17.317914
33.129116	1132.517900	17.322931
33.240865	1136.145454	17.327949
32.912076	1128.704976	17.332967
33.267641	1129.012227	17.337984
33.301999	1137.022782	17.343002
33.356539	1130.090300	17.348019
33.329648	1130.066146	17.353037
33.158072	1125.236186	17.358055
33.364349	1126.097013	17.363072
33.286656	1140.301157	17.368090
33.487858	1142.554518	17.373107
33.668076	1151.952900	17.378125
33.365036	1153.045009	17.383143
33.806916	1145.865637	17.388160
33.713046	1146.489463	17.393178
33.523016	1150.580877	17.398195
33.751600	1150.197953	17.403213
33.917698	1151.090323	17.408231
34.256789	1142.478512	17.413248
34.142883	1143.651442	17.418266
34.515329	1138.187121	17.423283
33.924439	1138.371257	17.428301
34.224183	1146.283431	17.433319
34.544129	1134.941640	17.438336
34.018071	1140.906636	17.443354
34.209394	1144.546971	17.448371
34.367810	1144.569525	17.453389
34.270228	1143.003759	17.458407
34.255198	1134.425344	17.463424
34.102868	1138.529784	17.468442
34.326224	1147.107191	17.473459
34.309369	1134.274950	17.478477
34.236224	1140.235257	17.483495
34.538700	1136.703823	17.488512
34.290235	1146.784763	17.493530
34.364186	1145.466682	17.498547
34.351969	1138.314277	17.503565
34.414621	1138.657954	17.508583
34.611394	1136.099310	17.513600
34.439767	1140.553919	17.518618
34.337680	1140.308012	17.523635
34.436797	1135.659704	17.528653
34.258128	1135.185951	17.533671
34.431005	1137.263864	17.538688
34.328751	1148.887208	17.543706
34.691617	1157.029343	17.548723
34.863307	1162.335902	17.553741
35.020627	1165.192601	17.558759
35.272313	1157.064703	17.563776
34.678008	1155.740867	17.568794
34.714121	1151.055088	17.573811
34.911253	1153.760377	17.578829
34.810543	1163.363731	17.583847
34.913539	1160.359018	17.588864
34.824513	1158.343777	17.593882
34.973469	1163.401429	17.598899
35.200772	1159.600896	17.603917
34.690838	1164.932199	17.608935
35.333506	1155.900424	17.613952
35.109585	1160.473687	17.618970
34.988082	1172.781731	17.623987
35.421125	1161.277033	17.629005
35.135661	1165.882031	17.634023
35.430698	1171.033565	17.639040
35.339310	1178.016090	17.644058
35.791456	1182.571798	17.649075
35.943305	1172.016888	17.654093
35.553023	1163.216379	17.659111
35.157121	1157.752512	17.664128
35.330749	1168.584702	17.669146
35.620319	1180.184546	17.674163
35.964688	1168.712672	17.679181
35.677318	1175.416627	17.684199
35.356543	1178.218845	17.689216
35.336382	1180.115565	17.694234
35.744953	1179.956910	17.699251
36.047353	1172.736263	17.704269
35.707614	1168.813127	17.709287
35.946733	1173.216013	17.714304
35.396113	1173.605283	17.719322
35.561437	1170.281527	17.724339
35.812155	1179.258615	17.729357
36.188141	1188.941933	17.734375
36.142564	1193.174829	17.739392
36.437685	1193.033950	17.744410
36.450293	1192.416614	17.749427
36.393298	1173.553440	17.754445
36.344970	1178.802957	17.759463
36.121184	1172.848204	17.764480
36.235426	1174.484019	17.769498
36.556101	1182.200421	17.774515
36.228121	1172.490723	17.779533
36.497342	1189.114757	17.784551
36.708597	1190.069484	17.789568
36.740747	1176.005054	17.794586
36.187439	1179.414918	17.799603
36.780501	1173.893929	17.804621
36.702856	1187.785672	17.809639
36.599737	1184.472414	17.814656
36.772785	1190.485685	17.819674
36.510787	1183.830000	17.824691
36.852202	1184.038481	17.829709
36.509630	1190.050486	17.834727
36.663309	1193.781938	17.839744
36.964764	1192.513418	17.844762
36.909895	1189.479785	17.849779
36.994836	1193.531283	17.854797
36.881464	1194.915577	17.859815
36.758626	1191.517043	17.864832
37.102275	1193.025396	17.869850
37.012776	1188.536017	17.874867
37.333450	1186.857378	17.879885
37.211548	1192.269907	17.884903
37.273655	1188.791903	17.889920
37.325123	1191.210744	17.894938
37.327656	1199.207379	17.899955
37.557570	1187.841790	17.904973
37.156743	1190.296782	17.909991
37.390538	1184.626947	17.915008
36.933700	1188.867473	17.920026
37.238612	1192.862415	17.925043
37.377624	1183.414065	17.930061
37.076488	1190.940711	17.935079
37.114696	1189.116975	17.940096
37.237170	1187.321063	17.945114
37.228197	1203.587902	17.950131
37.662765	1205.495431	17.955149
37.612733	1212.443088	17.960167
37.514181	1210.249448	17.965184
37.359802	1213.319097	17.970202
37.364895	1210.212948	17.975219
37.423554	1207.650685	17.980237
37.654583	1213.067886	17.985255
37.745176	1223.335593	17.990272
38.247275	1221.786320	17.995290
38.092359	1238.959704	18.000307
38.109344	1238.347992	18.005325
38.326108	1238.970490	18.010343
37.968729	1217.976772	18.015360
38.375026	1215.969127	18.020378
38.149698	1215.231276	18.025395
38.506935	1213.922455	18.030413
38.123470	1218.183051	18.035431
38.392102	1226.374697	18.040448
38.646338	1210.164158	18.045466
38.030550	1208.203040	18.050483
38.448520	1208.273292	18.055501
37.961779	1217.836169	18.060519
38.248394	1230.440079	18.065536
38.544884	1225.647212	18.070554
38.294545	1229.423037	18.075571
38.194006	1225.863209	18.080589
38.157089	1226.875755	18.085607
38.335342	1233.377388	18.090624
38.493852	1227.877129	18.095642
38.171729	1252.164840	18.100659
38.570830	1249.381971	18.105677
38.658639	1255.604284	18.110695
38.721470	1249.825512	18.115712
39.009479	1248.322403	18.120730
38.846715	1251.494361	18.125747
39.093603	1248.912069	18.130765
38.731086	1256.991171	18.135783
39.056588	1251.218582	18.140800
39.108191	1245.249061	18.145818
38.887692	1251.301922	18.150835
39.111833	1242.086364	18.155853
38.993812	1246.141270	18.160871
39.290165	1262.988347	18.165888
39.680961	1261.652174	18.170906
39.501004	1260.537973	18.175923
39.581518	1245.244582	18.180941
39.274941	1246.128962	18.185959
39.314696	1247.407215	18.190976
39.646502	1242.700331	18.195994
39.531651	1252.593133	18.201011
39.597836	1243.525402	18.206029
39.313186	1254.180131	18.211047
39.785885	1268.923009	18.216064
40.295994	1256.064923	18.221082
39.693966	1258.406276	18.226099
39.884208	1242.215203	18.231117
39.786208	1249.384989	18.236135
39.811677	1240.778086	18.241152
39.900204	1240.650640	18.246170
39.408678	1249.734589	18.251187
39.492881	1243.299201	18.256205
39.840158	1255.934652	18.261223
39.764332	1264.476938	18.266240
40.351436	1268.970497	18.271258
40.113781	1268.098872	18.276275
39.992246	1275.764675	18.281293
40.220595	1267.747684	18.286311
39.834359	1273.697128	18.291328
40.130664	1267.569336	18.296346
39.913606	1268.872048	18.301363
40.364065	1267.425539	18.306381
40.273627	1267.802672	18.311399
40.167325	1268.715636	18.316416
40.287168	1260.008728	18.321434
40.013073	1275.401963	18.326451
40.695085	1283.642480	18.331469
40.543455	1285.054867	18.336487
40.408571	1291.643453	18.341504
40.686997	1293.928917	18.346522
40.597007	1293.409705	18.351539
40.614915	1283.046133	18.356557
41.027442	1294.014543	18.361575
40.718650	1295.476801	18.366592
40.843562	1286.889011	18.371610
40.437254	1281.063808	18.376627
40.928992	1284.227902	18.381645
41.168350	1282.823934	18.386663
40.555864	1287.060466	18.391680
40.844360	1278.393399	18.396698
40.912322	1285.000695	18.401715
40.973602	1293.647750	18.406733
41.498087	1305.027828	18.411751
41.494614	1307.733012	18.416768
41.446658	1284.459516	18.421786
41.033167	1284.025705	18.426803
41.531544	1294.210627	18.431821
41.454865	1286.509669	18.436839
41.573589	1288.589773	18.441856
41.512101	1283.407997	18.446874
41.163836	1281.777350	18.451891
41.531658	1296.271588	18.456909
41.779035	1303.614508	18.461927
41.554628	1311.066064	18.466944
41.862882	1300.486573	18.471962
41.757700	1304.713055	18.476979
41.798297	1306.231029	18.481997
42.107131	1302.610201	18.487015
42.003271	1305.687730	18.492032
42.186330	1289.125344	18.497050
41.517764	1289.293247	18.502067
41.490176	1290.660952	18.507085
41.999164	1294.368315	18.512103
41.997507	1295.362718	18.517120
42.360472	1296.713415	18.522138
41.816320	1314.894625	18.527155
42.099041	1309.876669	18.532173
42.139985	1310.059643	18.537191
42.078548	1302.211119	18.542208
42.452119	1298.375016	18.547226
42.030550	1300.205249	18.552243
42.054867	1299.671284	18.557261
42.212600	1304.705510	18.562279
42.000607	1317.665322	18.567296
42.139456	1310.473400	18.572314
42.586030	1330.907353	18.577331
42.680525	1331.880381	18.582349
42.522941	1340.495475	18.587367
42.528378	1327.514431	18.592384
42.423545	1329.332912	18.597402
42.333476	1329.612155	18.602419
42.663595	1333.416982	18.607437
42.688409	1325.479192	18.612455
42.598834	1329.469698	18.617472
42.694045	1320.463654	18.622490
42.723493	1328.897956	18.627507
42.898468	1334.058881	18.632525
42.884780	1325.786286	18.637543
43.151493	1351.717621	18.642560
43.320379	1344.060217	18.647578
43.527390	1355.868777	18.652595
43.253568	1345.282624	18.657613
43.234868	1331.863531	18.662631
42.839310	1343.413031	18.667648
43.296890	1345.042407	18.672666
43.585107	1342.494653	18.677683
43.812863	1344.220000	18.682701
43.810830	1337.633983	18.687719
43.358175	1329.417538	18.692736
43.781610	1329.903515	18.697754
43.682515	1326.226671	18.702771
43.774191	1318.736014	18.707789
43.922719	1310.135045	18.712807
43.363426	1320.776037	18.717824
43.935006	1316.388184	18.722842
43.733837	1325.003787	18.727859
43.616056	1333.274961	18.732877
43.713867	1335.733900	18.737895
43.606592	1348.629988	18.742912
43.861551	1337.396085	18.747930
44.084772	1346.696312	18.752947
43.984706	1338.550857	18.757965
43.988939	1345.070328	18.762983
43.975821	1337.580303	18.768000
44.197560	1343.649115	18.773018
43.981624	1329.026969	18.778035
44.017767	1339.880804	18.783053
44.412850	1332.550894	18.788071
43.846102	1345.493722	18.793088
44.215988	1350.529437	18.798106
44.298152	1360.353560	18.803123
44.555347	1363.664873	18.808141
44.698073	1364.532514	18.813159
44.612395	1362.863874	18.818176
44.835140	1350.470480	18.823194
44.616374	1356.033939	18.828211
44.356140	1360.571915	18.833229
45.045542	1359.192107	18.838247
44.819031	1356.743933	18.843264
44.715163	1358.978845	18.848282
44.822468	1361.253258	18.853299
44.728126	1360.674764	18.858317
45.010263	1354.908936	18.863335
44.788194	1370.925283	18.868352
44.980183	1351.035112	18.873370
45.173176	1360.971264	18.878387
44.988102	1360.896151	18.883405
45.312201	1365.853834	18.888423
45.623400	1376.317447	18.893440
45.172915	1356.486904	18.898458
45.323607	1361.721071	18.903475
45.433317	1367.091053	18.908493
45.318568	1356.902862	18.913511
45.161185	1367.891180	18.918528
45.458724	1372.556371	18.923546
45.491496	1372.847928	18.928563
45.315623	1387.484231	18.933581
45.498091	1367.835382	18.938599
45.197573	1372.606898	18.943616
45.552246	1375.170770	18.948634
45.657794	1372.414939	18.953651
45.485055	1371.596256	18.958669
45.812692	1373.324891	18.963687
45.740170	1385.937842	18.968704
45.672614	1393.958169	18.973722
45.745000	1392.574041	18.978739
45.824675	1402.253406	18.983757
46.187670	1397.361708	18.988775
46.058154	1400.257074	18.993792
46.151455	1402.767223	18.998810
46.167027	1404.554223	19.003827
46.054939	1397.590937	19.008845
46.252063	1394.568282	19.013863
46.010524	1404.654593	19.018880
46.127907	1406.428798	19.023898
46.304843	1409.598055	19.028915
46.303329	1423.979843	19.033933
46.356033	1414.317669	19.038951
46.982233	1420.992193	19.043968
46.738395	1422.643107	19.048986
47.159488	1411.591418	19.054003
47.005242	1408.181984	19.059021
46.971826	1404.539017	19.064039
46.901240	1412.635569	19.069056
46.720823	1416.488843	19.074074
46.930134	1408.749336	19.079091
46.707269	1411.823437	19.084109
46.875652	1404.753087	19.089127
47.056772	1400.622056	19.094144
46.802443	1403.811543	19.099162
47.204848	1404.070434	19.104179
47.286468	1410.498906	19.109197
47.282118	1396.582038	19.114215
47.447754	1407.825895	19.119232
47.185576	1404.064129	19.124250
47.290876	1402.873667	19.129267
47.165452	1403.350961	19.134285
47.628094	1404.704985	19.139303
47.234813	1401.213079	19.144320
47.244239	1411.234826	19.149338
47.049939	1419.350764	19.154355
47.365290	1427.711915	19.159373
47.587898	1430.126067	19.164391
47.821315	1428.656744	19.169408
47.625567	1432.619725	19.174426
47.838237	1426.280913	19.179443
47.642727	1439.594850	19.184461
47.848599	1421.854763	19.189479
47.963477	1436.335095	19.194496
47.851561	1452.312165	19.199514
48.293913	1447.032465	19.204531
48.071451	1459.126141	19.209549
48.232158	1450.744110	19.214567
48.261542	1440.934091	19.219584
48.155818	1461.833438	19.224602
48.408823	1457.511243	19.229619
48.395925	1455.774385	19.234637
48.322062	1448.205465	19.239655
48.175240	1451.311842	19.244672
48.402538	1444.349014	19.249690
48.241129	1443.512772	19.254707
48.156646	1452.056505	19.259725
48.427668	1447.807232	19.264743
48.370947	1453.171757	19.269760
48.523376	1476.514386	19.274778
48.834583	1472.656458	19.279795
48.933224	1467.051893	19.284813
48.831615	1459.638800	19.289831
48.995317	1458.726372	19.294848
49.357341	1460.064606	19.299866
49.149099	1458.885394	19.304883
49.336837	1459.256818	19.309901
49.396904	1457.303393	19.314919
49.596793	1464.354007	19.319936
49.666641	1444.119938	19.324954
49.570249	1428.620568	19.329971
49.133608	1437.702324	19.334989
49.464301	1431.411293	19.340007
49.370348	1435.604488	19.345024
49.488606	1423.454640	19.350042
49.774306	1422.756638	19.355059
49.391284	1430.785381	19.360077
49.612439	1422.864124	19.365095
49.610284	1423.786026	19.370112
49.645917	1442.498243	19.375130
50.165726	1440.204536	19.380147
49.438912	1445.926520	19.385165
50.018405	1440.063581	19.390183
49.974765	1448.108589	19.395200
49.598640	1448.110748	19.400218
50.058622	1445.182605	19.405235
49.705768	1457.183096	19.410253
49.801016	1458.152857	19.415271
49.893158	1454.651160	19.420288
49.739501	1454.331274	19.425306
49.791648	1459.887035	19.430323
50.311317	1476.033425	19.435341
49.968848	1476.238603	19.440359
50.279288	1477.979411	19.445376
50.208812	1483.503896	19.450394
50.622433	1475.874367	19.455411
50.551742	1484.605309	19.460429
50.492203	1484.920798	19.465447
50.634078	1487.073042	19.470464
50.494143	1480.246635	19.475482
50.830943	1484.179841	19.480499
50.958838	1498.907503	19.485517
50.901992	1500.674299	19.490535
50.969554	1509.156365	19.495552
50.911773	1508.521644	19.500570
51.264764	1507.847811	19.505587
51.277848	1501.366667	19.510605
51.302952	1502.893397	19.515623
51.632645	1494.121938	19.520640
50.910835	1493.240946	19.525658
50.966813	1479.383991	19.530675
51.133966	1504.264444	19.535693
51.125914	1498.818602	19.540711
51.219911	1498.873341	19.545728
51.219717	1499.289990	19.550746
51.559753	1498.889598	19.555763
51.530795	1494.021412	19.560781
51.287025	1498.941867	19.565799
51.368835	1498.799692	19.570816
51.290367	1510.264903	19.575834
51.582192	1521.678417	19.580851
51.583788	1527.276834	19.585869
51.735548	1526.965902	19.590887
51.720907	1511.624073	19.595904
51.717136	1522.187615	19.600922
52.187032	1514.397767	19.605939
51.931780	1526.682826	19.610957
52.006569	1520.927340	19.615975
52.172055	1521.794578	19.620992
51.979004	1525.479434	19.626010
51.737034	1529.364468	19.631027
52.057834	1539.233356	19.636045
52.109817	1539.348329	19.641063
52.320541	1539.690906	19.646080
51.982876	1540.962039	19.651098
52.602440	1541.931711	19.656115
52.526564	1549.495800	19.661133
52.102419	1544.468602	19.666151
53.007642	1551.424521	19.671168
52.490490	1568.105841	19.676186
52.985767	1562.972457	19.681203
52.851706	1566.616520	19.686221
53.124557	1563.850227	19.691239
53.105975	1564.295007	19.696256
53.302850	1568.619399	19.701274
53.585366	1563.617184	19.706291
53.411517	1547.912087	19.711309
53.175268	1533.513871	19.716327
53.201835	1529.763646	19.721344
53.150574	1526.555813	19.726362
53.402446	1540.964271	19.731379
53.337284	1541.413192	19.736397
53.604290	1550.125973	19.741415
53.472892	1548.868440	19.746432
53.386972	1558.999886	19.751450
53.695304	1554.498579	19.756467
53.769964	1558.829494	19.761485
53.635701	1561.593080	19.766503
54.054678	1553.309399	19.771520
53.675628	1557.222227	19.776538
53.690720	1544.160614	19.781555
53.305439	1546.436484	19.786573
53.511568	1554.262518	19.791591
53.581819	1547.753464	19.796608
53.697167	1560.659009	19.801626
54.021059	1575.034120	19.806643
54.299630	1573.652390	19.811661
54.151456	1571.333930	19.816679
54.186903	1575.251252	19.821696
54.184212	1581.090209	19.826714
54.060821	1573.434317	19.831731
54.136754	1584.619753	19.836749
54.334008	1583.276010	19.841767
54.806814	1588.267264	19.846784
54.686932	1601.796700	19.851802
54.780616	1603.120180	19.856819
54.901349	1600.343000	19.861837
54.472938	1596.572523	19.866855
54.649987	1592.906010	19.871872
54.958515	1602.546472	19.876890
55.105658	1601.860704	19.881907
55.481393	1601.009728	19.886925
55.083519	1594.706551	19.891943
55.576523	1591.568075	19.896960
55.423233	1590.506482	19.901978
55.383351	1582.913244	19.906995
55.144424	1567.669626	19.912013
54.915713	1573.443003	19.917031
55.470393	1590.530796	19.922048
55.489007	1596.066605	19.927066
55.803015	1586.628497	19.932083
55.387663	1583.872192	19.937101
55.507640	1588.375903	19.942119
55.858498	1577.028990	19.947136
55.502573	1582.333129	19.952154
55.419067	1584.214569	19.957171
55.693243	1585.642320	19.962189
55.858827	1589.312027	19.967207
55.845946	1581.559919	19.972224
55.579064	1589.747268	19.977242
55.694515	1587.920858	19.982259
55.941926	1586.045369	19.987277
56.071950	1589.045275	19.992295
56.110971	1593.719469	19.997312
55.779074	1608.440360	20.002330
55.990357	1610.023140	20.007347
56.087777	1610.285637	20.012365
55.855748	1622.693361	20.017383
56.187928	1611.955295	20.022400
56.532636	1625.730711	20.027418
56.209550	1627.955819	20.032435
56.822956	1637.422294	20.037453
56.744659	1630.381036	20.042471
56.868699	1632.529779	20.047488
56.830415	1638.620497	20.052506
56.944353	1631.915210	20.057523
57.133028	1631.282898	20.062541
56.791184	1638.759301	20.067559
56.768709	1629.683173	20.072576
56.973785	1634.706919	20.077594
57.185347	1630.605782	20.082611
57.150999	1626.259137	20.087629
56.939558	1644.707305	20.092647
57.488793	1620.778044	20.097664
57.418141	1626.864361	20.102682
57.256820	1635.666384	20.107699
57.515791	1630.759362	20.112717
57.324291	1634.324071	20.117735
57.693216	1645.820263	20.122752
57.384355	1656.769372	20.127770
57.582425	1666.405083	20.132787
57.745172	1657.590270	20.137805
57.700012	1660.980570	20.142823
58.071881	1656.762788	20.147840
58.105898	1647.942900	20.152858
58.434594	1652.940972	20.157875
58.009150	1652.193427	20.162893
58.070895	1659.496147	20.167911
57.610157	1648.361558	20.172928
58.254235	1648.200719	20.177946
57.849763	1651.874542	20.182963
58.101594	1653.558276	20.187981
58.405485	1664.790102	20.192999
58.584426	1667.176413	20.198016
58.348009	1663.997565	20.203034
58.160453	1669.073368	20.208051
58.569251	1666.210018	20.213069
58.889396	1667.157178	20.218087
58.612202	1659.424356	20.223104
58.563095	1663.869366	20.228122
58.164551	1664.660871	20.233139
58.663118	1661.950722	20.238157
58.945214	1680.665601	20.243175
59.071080	1684.934873	20.248192
59.186757	1676.250508	20.253210
58.879874	1683.023983	20.258227
59.355763	1685.717240	20.263245
59.271150	1683.401431	20.268263
59.325112	1677.425084	20.273280
59.699484	1686.155826	20.278298
59.293534	1684.875023	20.283315
59.471267	1671.731027	20.288333
59.391749	1678.667705	20.293351
59.738653	1676.098086	20.298368
59.325218	1674.831081	20.303386
59.290730	1677.601144	20.308403
59.434716	1679.816199	20.313421
59.471519	1699.184942	20.318439
59.468169	1704.206647	20.323456
59.666195	1698.337117	20.328474
60.264025	1715.475077	20.333491
60.104522	1707.389261	20.338509
59.839309	1706.458811	20.343527
60.156102	1702.148656	20.348544
60.433741	1704.570004	20.353562
60.320376	1700.144198	20.358579
60.397316	1698.424801	20.363597
60.150621	1709.386294	20.368615
60.288632	1715.219031	20.373632
60.469930	1723.579232	20.378650
60.319192	1724.884209	20.383667
60.787946	1707.667572	20.388685
60.994930	1722.133706	20.393703
60.957276	1718.841651	20.398720
61.391826	1726.448926	20.403738
60.726372	1728.803431	20.408755
61.119655	1723.648110	20.413773
60.875270	1719.305947	20.418791
60.660867	1723.158299	20.423808
60.926182	1720.528870	20.428826
60.897045	1724.349041	20.433843
61.145283	1731.729875	20.438861
61.436540	1734.480470	20.443879
61.453022	1737.229933	20.448896
61.486310	1748.245418	20.453914
61.578304	1748.256289	20.458931
61.486160	1738.562982	20.463949
61.251795	1742.383750	20.468967
61.725396	1732.358799	20.473984
61.769129	1731.029630	20.479002
61.454061	1740.064086	20.484019
61.755587	1744.286915	20.489037
62.086292	1753.611542	20.494055
62.303782	1748.988713	20.499072
62.173976	1756.289924	20.504090
62.146439	1762.464212	20.509107
62.262309	1753.609356	20.514125
62.474513	1751.868761	20.519143
62.270418	1759.033282	20.524160
62.195859	1762.245161	20.529178
62.346971	1755.341490	20.534195
62.575016	1754.822932	20.539213
62.614722	1757.704467	20.544231
62.375830	1756.473228	20.549248
62.506922	1759.267857	20.554266
62.365039	1754.398357	20.559283
62.837184	1758.187336	20.564301
62.708381	1773.523519	20.569319
62.720161	1779.480201	20.574336
62.765574	1784.194471	20.579354
62.795917	1779.518899	20.584371
62.993317	1779.611091	20.589389
63.107962	1778.763142	20.594407
63.046468	1776.784544	20.599424
62.920638	1775.491406	20.604442
63.320894	1794.645509	20.609459
63.579215	1793.405799	20.614477
63.717646	1803.319186	20.619495
63.590641	1805.655614	20.624512
63.782126	1812.663499	20.629530
63.759013	1804.007129	20.634547
64.460995	1797.907122	20.639565
64.094063	1797.200899	20.644583
63.615215	1772.469936	20.649600
63.945134	1781.236093	20.654618
63.735376	1795.022767	20.659635
63.931513	1803.197634	20.664653
63.845651	1801.024024	20.669671
63.580389	1808.939804	20.674688
63.973624	1797.911180	20.679706
63.975244	1798.759922	20.684723
64.185084	1811.792863	20.689741
64.079855	1817.158785	20.694759
63.968925	1822.172131	20.699776
64.778524	1810.664830	20.704794
64.273974	1822.591495	20.709811
64.453537	1820.540409	20.714829
64.633012	1822.084008	20.719847
64.745589	1838.622732	20.724864
64.915523	1851.769259	20.729882
64.701498	1851.865947	20.734899
65.039781	1844.762492	20.739917
64.889021	1838.840259	20.744935
65.002357	1846.381140	20.749952
64.869431	1844.748262	20.754970
64.948752	1847.030277	20.759987
65.098213	1853.902743	20.765005
65.350493	1866.458831	20.770023
65.318925	1859.968773	20.775040
65.904126	1857.743670	20.780058
65.514828	1869.712273	20.785075
65.685561	1859.895658	20.790093
65.561378	1857.226242	20.795111
65.726908	1868.072750	20.800128
66.170010	1860.949711	20.805146
66.179423	1859.032583	20.810163
66.433772	1857.411615	20.815181
66.477636	1847.917859	20.820199
66.115511	1860.668042	20.825216
66.232664	1844.550995	20.830234
66.117384	1850.357184	20.835251
66.325752	1847.749283	20.840269
66.379784	1853.390083	20.845287
66.705745	1849.570792	20.850304
66.675296	1856.865946	20.855322
66.318197	1849.091908	20.860339
66.558138	1871.799612	20.865357
66.819808	1870.707704	20.870375
66.905070	1884.615492	20.875392
67.176667	1873.498575	20.880410
67.009236	1868.863435	20.885427
67.202410	1871.645199	20.890445
67.223820	1872.232052	20.895463
66.992274	1872.536625	20.900480
66.839018	1860.918199	20.905498
67.256719	1873.618800	20.910515
67.403567	1861.148576	20.915533
67.418996	1858.952778	20.920551
67.473484	1856.416325	20.925568
67.495880	1861.654960	20.930586
67.755155	1864.072895	20.935603
67.522842	1865.056128	20.940621
67.772971	1863.117065	20.945639
67.525872	1865.039945	20.950656
67.591463	1860.810137	20.955674
67.560283	1878.327687	20.960691
67.712998	1884.893524	20.965709
67.765084	1887.375483	20.970727
67.854142	1886.638842	20.975744
68.488263	1884.238803	20.980762
68.033865	1889.861436	20.985779
67.811864	1882.182989	20.990797
68.043658	1898.112918	20.995815
68.340668	1913.739135	21.000832
68.627749	1908.196432	21.005850
68.792561	1915.997539	21.010867
68.564739	1908.209532	21.015885
68.658734	1906.787264	21.020903
68.726239	1910.055811	21.025920
68.634164	1908.766843	21.030938
69.106926	1906.650875	21.035955
68.978949	1902.378797	21.040973
68.935868	1897.758882	21.045991
68.827432	1906.325519	21.051008
69.213215	1912.144749	21.056026
69.536100	1923.458974	21.061043
69.435542	1923.108668	21.066061
69.413441	1923.538228	21.071079
69.419744	1932.970583	21.076096
70.226424	1928.627806	21.081114
69.811284	1922.178885	21.086131
69.643834	1923.773691	21.091149
69.729128	1926.935307	21.096167
69.718957	1930.212872	21.101184
69.935634	1929.585631	21.106202
69.776764	1925.984305	21.111219
70.026637	1924.992078	21.116237
70.088516	1920.709186	21.121255
69.885789	1933.027321	21.126272
70.141486	1930.856990	21.131290
69.861335	1929.644827	21.136307
69.729481	1947.014105	21.141325
70.256149	1942.648919	21.146343
70.178120	1953.650411	21.151360
70.361430	1950.740288	21.156378
70.752375	1963.975355	21.161395
70.689869	1962.946856	21.166413
71.077592	1958.909568	21.171431
71.167493	1966.107011	21.176448
71.557547	1959.333094	21.181466
71.222554	1956.687223	21.186483
71.158647	1962.094054	21.191501
71.193603	1960.589507	21.196519
71.264092	1974.345035	21.201536
71.296028	1957.086137	21.206554
71.436724	1963.335128	21.211571
71.411863	1962.871969	21.216589
71.431885	1959.826470	21.221607
71.395491	1947.599505	21.226624
71.426131	1949.598807	21.231642
71.212720	1951.658439	21.236659
71.484816	1946.821863	21.241677
72.023175	1966.093378	21.246695
71.990830	1972.479944	21.251712
72.137950	1976.140000	21.256730
71.994387	1978.460108	21.261747
71.832456	1977.131583	21.266765
72.294767	1973.713810	21.271783
72.247985	1984.186527	21.276800
72.017740	1975.893908	21.281818
72.111851	1972.107760	21.286835
72.169527	1987.342320	21.291853
72.323070	1994.823313	21.296871
72.374757	2005.798202	21.301888
72.788230	1998.133759	21.306906
72.755698	1998.268289	21.311923
72.700097	2003.301421	21.316941
72.880436	1994.584679	21.321959
72.817934	2005.940400	21.326976
72.988169	1999.270341	21.331994
73.206499	2007.309272	21.337011
72.670249	2018.915963	21.342029
73.130291	2021.962074	21.347047
73.293547	2025.190393	21.352064
73.388265	2025.106156	21.357082
73.444258	2022.982883	21.362099
73.351282	2027.122410	21.367117
73.285563	2019.911758	21.372135
73.543613	2038.258369	21.377152
73.787256	2037.554311	21.382170
73.955902	2037.909803	21.387187
73.978149	2053.276212	21.392205
74.097839	2047.908026	21.397223
73.795234	2045.010897	21.402240
73.862972	2040.764931	21.407258
73.820827	2033.629481	21.412275
74.120133	2050.451592	21.417293
74.118721	2055.015468	21.422311
74.072813	2065.661676	21.427328
74.179244	2063.947092	21.432346
74.497486	2060.419321	21.437363
74.318569	2068.485802	21.442381
74.803786	2076.107381	21.447399
74.955328	2086.097772	21.452416
75.235158	2087.385813	21.457434
75.253810	2087.720623	21.462451
75.219046	2085.482164	21.467469
75.602168	2078.911275	21.472487
75.550860	2077.922043	21.477504
75.548623	2077.512144	21.482522
75.629070	2074.987374	21.487539
75.604926	2066.252137	21.492557
75.678255	2052.107979	21.497575
75.868089	2069.067188	21.502592
75.664927	2070.490864	21.507610
75.864607	2072.031320	21.512627
75.676400	2070.681656	21.517645
75.861682	2072.599935	21.522663
76.175031	2076.085635	21.527680
76.108401	2071.762876	21.532698
76.151773	2073.943248	21.537715
75.924500	2081.919473	21.542733
76.036610	2083.378969	21.547751
76.104466	2072.274914	21.552768
76.239350	2070.284452	21.557786
76.675699	2082.483627	21.562803
76.261850	2103.766537	21.567821
76.530367	2090.074642	21.572839
76.781683	2099.462386	21.577856
76.902798	2097.231064	21.582874
77.177217	2092.892739	21.587891
76.770111	2104.532904	21.592909
76.779867	2098.727457	21.597927
76.876218	2101.363469	21.602944
77.032108	2099.458083	21.607962
77.390601	2104.117073	21.612979
77.210958	2117.690978	21.617997
77.344036	2115.038026	21.623015
77.783443	2124.333193	21.628032
77.805813	2123.856318	21.633050
77.760917	2120.297060	21.638067
77.612717	2120.345564	21.643085
77.757408	2112.631659	21.648103
78.050740	2112.992866	21.653120
77.845204	2106.552067	21.658138
78.162783	2101.159173	21.663155
77.923074	2116.052243	21.668173
77.974887	2114.384083	21.673191
78.076276	2113.143691	21.678208
77.620487	2113.808472	21.683226
78.153224	2125.983107	21.688243
77.999423	2143.002537	21.693261
78.097257	2138.612966	21.698279
78.450124	2137.219554	21.703296
78.252220	2145.216454	21.708314
78.902651	2157.918668	21.713331
78.804082	2155.074768	21.718349
78.640101	2159.973433	21.723367
79.137444	2155.543358	21.728384
78.760048	2157.546648	21.733402
79.094942	2153.637524	21.738419
78.640898	2165.764802	21.743437
79.097031	2168.536974	21.748455
79.688393	2180.573064	21.753472
79.408905	2172.878250	21.758490
79.672333	2167.878859	21.763507
79.451737	2171.041102	21.768525
79.769651	2171.392148	21.773543
80.002396	2167.284414	21.778560
79.898068	2182.582395	21.783578
79.805396	2179.911149	21.788595
79.812035	2184.827275	21.793613
80.064505	2190.632766	21.798631
80.403357	2199.968976	21.803648
80.725205	2203.352376	21.808666
80.425049	2196.819062	21.813683
80.308411	2201.050706	21.818701
80.735427	2196.675824	21.823719
80.374903	2190.783182	21.828736
80.692894	2189.275300	21.833754
80.661799	2190.807738	21.838771
80.714654	2195.817619	21.843789
80.942034	2200.093202	21.848807
80.959762	2211.894112	21.853824
81.172766	2214.148918	21.858842
81.280955	2219.610921	21.863859
81.237338	2215.202465	21.868877
81.318226	2214.151484	21.873895
81.256093	2218.996336	21.878912
81.217100	2211.535248	21.883930
81.538827	2215.379453	21.888947
81.284486	2225.124219	21.893965
81.618187	2235.578500	21.898983
82.093705	2244.255796	21.904000
81.821375	2244.462614	21.909018
82.165023	2241.006574	21.914035
82.421912	2235.203392	21.919053
82.227092	2238.519412	21.924071
82.367168	2235.982120	21.929088
82.346579	2245.564032	21.934106
82.446560	2237.954916	21.939123
82.377548	2253.777643	21.944141
82.371147	2241.394287	21.949159
82.293023	2241.677984	21.954176
82.461564	2253.584692	21.959194
82.790956	2258.769034	21.964211
82.727500	2262.197031	21.969229
82.445257	2254.875029	21.974247
82.764028	2259.079498	21.979264
82.647126	2259.776404	21.984282
82.805529	2263.324289	21.989299
82.962396	2286.184402	21.994317
83.314365	2272.501386	21.999335
83.513463	2271.589686	22.004352
83.129879	2267.786792	22.009370
83.468797	2270.804583	22.014387
83.463013	2281.974853	22.019405
83.819977	2292.709569	22.024423
84.224610	2291.232289	22.029440
83.842566	2301.868180	22.034458
83.908945	2289.022070	22.039475
84.020661	2298.974635	22.044493
84.245680	2295.799124	22.049511
84.344498	2287.738851	22.054528
84.091288	2297.780150	22.059546
84.354781	2289.457370	22.064563
84.437544	2308.377721	22.069581
84.691455	2313.450818	22.074599
85.060550	2311.467821	22.079616
84.584282	2313.095264	22.084634
84.826957	2306.237001	22.089651
84.946356	2315.566625	22.094669
85.162305	2316.643766	22.099687
85.075815	2315.492761	22.104704
85.158148	2307.709640	22.109722
85.327855	2307.885076	22.114739
85.169674	2315.061561	22.119757
85.346535	2326.146434	22.124775
85.395855	2328.613108	22.129792
85.530171	2347.430740	22.134810
85.460019	2336.897302	22.139827
85.521660	2334.596367	22.144845
85.362226	2344.705057	22.149863
85.671134	2353.900860	22.154880
85.907302	2361.340656	22.159898
86.369943	2352.841466	22.164915
86.557751	2364.685264	22.169933
86.282427	2355.266496	22.174951
86.597928	2358.117543	22.179968
86.391501	2361.347033	22.184986
86.384180	2358.709729	22.190003
86.904260	2375.734264	22.195021
86.611760	2380.791992	22.200039
87.261014	2380.305265	22.205056
87.080822	2385.342243	22.210074
87.023547	2384.312899	22.215091
87.043768	2375.955604	22.220109
86.937081	2378.014343	22.225127
87.465003	2378.928992	22.230144
87.466319	2387.440790	22.235162
87.525254	2371.960453	22.240179
87.848092	2380.870039	22.245197
87.692177	2378.167643	22.250215
87.659462	2367.337962	22.255232
87.568280	2372.364147	22.260250
87.889804	2389.028447	22.265267
87.797607	2386.467560	22.270285
87.706238	2389.729526	22.275303
88.295491	2383.599645	22.280320
87.880628	2396.816101	22.285338
87.997713	2389.624002	22.290355
88.355471	2391.306992	22.295373
87.931783	2409.994344	22.300391
88.237159	2401.472429	22.305408
88.340036	2410.514331	22.310426
88.133151	2418.074062	22.315443
88.659497	2432.194062	22.320461
88.782674	2434.614462	22.325479
88.876434	2432.614624	22.330496
89.251780	2432.890400	22.335514
89.177803	2430.216188	22.340531
89.276880	2429.335930	22.345549
89.513612	2427.108547	22.350567
89.502389	2424.156236	22.355584
89.556798	2423.926821	22.360602
89.833393	2428.522982	22.365619
89.732533	2427.898132	22.370637
89.595154	2444.751157	22.375655
89.986329	2440.085160	22.380672
89.917059	2448.724822	22.385690
89.850418	2454.671922	22.390707
90.229292	2448.322492	22.395725
90.314083	2452.936086	22.400743
89.970436	2451.506594	22.405760
90.295069	2458.329756	22.410778
90.548640	2459.823930	22.415795
91.376764	2469.617007	22.420813
90.729047	2473.259669	22.425831
91.050356	2460.875317	22.430848
91.046717	2470.533596	22.435866
91.090658	2460.682864	22.440883
91.085211	2464.341675	22.445901
91.138249	2477.327078	22.450919
91.360930	2464.099715	22.455936
91.439385	2466.640746	22.460954
91.302844	2458.948661	22.465971
91.170490	2468.955340	22.470989
90.918853	2471.772171	22.476007
91.753679	2482.697247	22.481024
91.484237	2498.254916	22.486042
91.500997	2492.760699	22.491059
91.783195	2479.530312	22.496077
91.839193	2497.710216	22.501095
92.256559	2501.574217	22.506112
92.307901	2512.824052	22.511130
92.211913	2511.216885	22.516147
92.624859	2513.023798	22.521165
92.251060	2514.616267	22.526183
92.524131	2513.232173	22.531200
92.436443	2513.189137	22.536218
92.819938	2527.738732	22.541235
93.130935	2531.070241	22.546253
92.753616	2535.213404	22.551271
92.967124	2526.658482	22.556288
93.037651	2533.089096	22.561306
93.402224	2531.848471	22.566323
93.512088	2532.263682	22.571341
93.332377	2540.387307	22.576359
93.465500	2549.636000	22.581376
93.460822	2558.593831	22.586394
93.371828	2557.957649	22.591411
94.064537	2550.959352	22.596429
93.767143	2551.892850	22.601447
94.032702	2551.860749	22.606464
93.953200	2560.874489	22.611482
94.344702	2575.659578	22.616499
94.275742	2569.998868	22.621517
94.220169	2576.887955	22.626535
94.823529	2577.844450	22.631552
94.824523	2575.458302	22.636570
94.573695	2580.493776	22.641587
95.145452	2571.784866	22.646605
94.875153	2576.867576	22.651623
94.735766	2571.015908	22.656640
94.819642	2578.318692	22.661658
94.604683	2584.276448	22.666675
95.416845	2583.716853	22.671693
95.223463	2594.815713	22.676711
95.259835	2588.778696	22.681728
95.398726	2585.424105	22.686746
95.603853	2584.233707	22.691763
95.815301	2584.932835	22.696781
95.968757	2579.590762	22.701799
96.047689	2582.251667	22.706816
95.860758	2585.575982	22.711834
96.092403	2574.518547	22.716851
96.474153	2585.735599	22.721869
96.320034	2594.814701	22.726887
96.319284	2598.267655	22.731904
96.651414	2587.554267	22.736922
96.551713	2588.024405	22.741939
96.726530	2589.969629	22.746957
96.758399	2598.921755	22.751975
96.580999	2595.578842	22.756992
96.642633	2597.147284	22.762010
96.921377	2605.158083	22.767027
97.437556	2607.176073	22.772045
97.166242	2622.402750	22.777063
97.309602	2617.807094	22.782080
97.446566	2617.668894	22.787098
97.487465	2620.316827	22.792115
97.966918	2620.778289	22.797133
97.558017	2619.892393	22.802151
97.406949	2627.569712	22.807168
97.538371	2629.111442	22.812186
97.487127	2638.881422	22.817203
97.920247	2640.969240	22.822221
97.984604	2647.776441	22.827239
97.981827	2655.711435	22.832256
98.181716	2659.445425	22.837274
98.536385	2671.405309	22.842291
98.860178	2664.123904	22.847309
98.876004	2669.259653	22.852327
98.714568	2668.177176	22.857344
98.921086	2662.716301	22.862362
98.706280	2669.213760	22.867379
98.912821	2676.955006	22.872397
98.898479	2683.872392	22.877415
99.401964	2676.026286	22.882432
99.235769	2689.377584	22.887450
99.063625	2693.040465	22.892467
99.421385	2701.600721	22.897485
99.583786	2716.630125	22.902503
99.662326	2713.663703	22.907520
100.043234	2706.919346	22.912538
99.826971	2716.327016	22.917555
100.213635	2713.672121	22.922573
100.187070	2720.029641	22.927591
100.218665	2734.874405	22.932608
100.330653	2739.812050	22.937626
100.406893	2743.798985	22.942643
100.805771	2737.020240	22.947661
100.722371	2739.293146	22.952679
100.393729	2729.399643	22.957696
101.103383	2728.098629	22.962714
100.817217	2735.835034	22.967731
101.099004	2745.893760	22.972749
101.198354	2746.831388	22.977767
101.551856	2751.734356	22.982784
101.442221	2748.986779	22.987802
101.164597	2751.391112	22.992819
101.400598	2751.723443	22.997837
101.691271	2752.132425	23.002855
101.574038	2754.536879	23.007872
101.801199	2763.575268	23.012890
101.993636	2766.833868	23.017907
101.836136	2773.262419	23.022925
101.981492	2775.366931	23.027943
102.186155	2782.385758	23.032960
102.467111	2772.952209	23.037978
102.226765	2776.452204	23.042995
102.572376	2779.402754	23.048013
102.975096	2789.953856	23.053031
102.794104	2788.012805	23.058048
103.074425	2791.604818	23.063066
103.295110	2790.090040	23.068083
103.078943	2789.041380	23.073101
103.143938	2793.721286	23.078119
103.364546	2791.720472	23.083136
103.651724	2785.448414	23.088154
103.198223	2791.244772	23.093171
103.424945	2791.546996	23.098189
103.312030	2809.463312	23.103207
103.346361	2809.432720	23.108224
103.483222	2806.091031	23.113242
103.907751	2832.867733	23.118259
103.935770	2830.287947	23.123277
104.054952	2843.070726	23.128295
104.067007	2850.833049	23.133312
104.527472	2842.286630	23.138330
104.534110	2843.147260	23.143347
104.682168	2853.956073	23.148365
105.135508	2869.706973	23.153383
104.970518	2864.610389	23.158400
105.230960	2858.172062	23.163418
104.846664	2863.184338	23.168435
105.035785	2862.397263	23.173453
105.227876	2859.728645	23.178471
105.491065	2860.407054	23.183488
105.441802	2858.088710	23.188506
105.554227	2876.051847	23.193523
105.884102	2886.336675	23.198541
106.021208	2890.841188	23.203559
105.950285	2883.116548	23.208576
106.409089	2883.669625	23.213594
106.177621	2875.174785	23.218611
106.188522	2871.354142	23.223629
106.191979	2873.660799	23.228647
106.021571	2872.557623	23.233664
106.529693	2887.106922	23.238682
106.673983	2897.120995	23.243699
107.145866	2897.807740	23.248717
107.419577	2901.811114	23.253735
106.726433	2895.537953	23.258752
107.226084	2900.957771	23.263770
106.975096	2898.374344	23.268787
107.279488	2895.940621	23.273805
107.353105	2897.485119	23.278823
107.237552	2915.543981	23.283840
107.521044	2913.236620	23.288858
107.518409	2919.177002	23.293875
107.504399	2904.484056	23.298893
107.688150	2918.074223	23.303911
107.903873	2937.605642	23.308928
108.095659	2927.005570	23.313946
108.065022	2933.811982	23.318963
108.241877	2931.486607	23.323981
108.495701	2937.225851	23.328999
108.256092	2955.692399	23.334016
108.788167	2950.344554	23.339034
108.842811	2966.754523	23.344051
108.844643	2971.242374	23.349069
108.646841	2961.874266	23.354087
108.874444	2964.489842	23.359104
108.908843	2956.417269	23.364122
108.533815	2982.205327	23.369139
108.882357	2982.308566	23.374157
108.875281	2988.795688	23.379175
109.132881	3007.073925	23.384192
109.754954	2996.346432	23.389210
109.585108	2994.113242	23.394227
109.810305	3011.159331	23.399245
109.897830	3013.528584	23.404263
110.062046	3030.502184	23.409280
110.432491	3021.641539	23.414298
110.576798	3027.994491	23.419315
110.555872	3021.148851	23.424333
110.410892	3026.246771	23.429351
110.322207	3038.011239	23.434368
111.392895	3042.659897	23.439386
111.080318	3049.542086	23.444403
111.125361	3041.341559	23.449421
111.473914	3046.990248	23.454439
110.985183	3044.131583	23.459456
111.109294	3042.149016	23.464474
111.631407	3047.764200	23.469491
111.686033	3059.724009	23.474509
111.778400	3064.806848	23.479527
111.656223	3067.897015	23.484544
112.197176	3064.902277	23.489562
112.356220	3067.216145	23.494579
112.372023	3070.691846	23.499597
112.593037	3061.273851	23.504615
112.453435	3060.099556	23.509632
112.535429	3056.864259	23.514650
112.872853	3071.951757	23.519667
112.662387	3085.338690	23.524685
112.783931	3086.354921	23.529703
112.648178	3089.024286	23.534720
112.862226	3092.257467	23.539738
113.198039	3101.376846	23.544755
113.013822	3106.294718	23.549773
113.740259	3112.771121	23.554791
113.727898	3114.654198	23.559808
113.605263	3106.262133	23.564826
113.663706	3113.581745	23.569843
113.511862	3099.702444	23.574861
114.112873	3119.157917	23.579879
113.966403	3135.564829	23.584896
114.268887	3139.320720	23.589914
114.398622	3125.454097	23.594931
114.308486	3122.804407	23.599949
114.460581	3126.413421	23.604967
114.636581	3140.771931	23.609984
114.697167	3143.164359	23.615002
115.123776	3153.863431	23.620019
115.227830	3151.606247	23.625037
115.275205	3140.454242	23.630055
115.212388	3146.429377	23.635072
115.134473	3144.986602	23.640090
115.608564	3157.543565	23.645107
115.907840	3162.164769	23.650125
115.959344	3161.134119	23.655143
115.829580	3158.661068	23.660160
116.085190	3163.412206	23.665178
116.114908	3158.079879	23.670195
116.206353	3160.309664	23.675213
116.483947	3156.147337	23.680231
116.514785	3155.198831	23.685248
116.502022	3156.176139	23.690266
116.743985	3155.737427	23.695283
116.660934	3170.976102	23.700301
116.638131	3176.859760	23.705319
116.570385	3177.732059	23.710336
116.875698	3178.829973	23.715354
117.101147	3182.351756	23.720371
117.379669	3192.152434	23.725389
117.425691	3192.896442	23.730407
117.634094	3200.375656	23.735424
117.594873	3193.141444	23.740442
117.893989	3188.685366	23.745459
117.808435	3194.821890	23.750477
118.208286	3192.581483	23.755495
118.063971	3196.337949	23.760512
118.297719	3209.339756	23.765530
118.339418	3218.091807	23.770547
118.210404	3220.526574	23.775565
118.412840	3214.507519	23.780583
118.635602	3218.490541	23.785600
118.803865	3231.875059	23.790618
118.939003	3231.573018	23.795635
119.053092	3234.683011	23.800653
119.206297	3226.033050	23.805671
119.354302	3244.240324	23.810688
119.223675	3243.487547	23.815706
119.367019	3249.430417	23.820723
119.314382	3254.706464	23.825741
119.303853	3266.604024	23.830759
119.388791	3279.714414	23.835776
120.068949	3283.045042	23.840794
120.206974	3289.367508	23.845811
120.379621	3299.970737	23.850829
120.586915	3289.797273	23.855847
120.257429	3301.826889	23.860864
120.715240	3305.934075	23.865882
121.004551	3313.615285	23.870899
120.369710	3318.660626	23.875917
121.028693	3318.825702	23.880935
121.165695	3315.865803	23.885952
121.316860	3315.573875	23.890970
121.633839	3327.126634	23.895987
121.126422	3335.939520	23.901005
121.667414	3334.415548	23.906023
121.591036	3341.649061	23.911040
121.678993	3336.967216	23.916058
122.064233	3336.392427	23.921075
121.859151	3352.458374	23.926093
122.092247	3346.683816	23.931111
121.787001	3353.830097	23.936128
122.321198	3370.174771	23.941146
122.439837	3376.585524	23.946163
122.444601	3388.247204	23.951181
122.854080	3373.610624	23.956199
123.239305	3379.054828	23.961216
123.205081	3372.084887	23.966234
123.635022	3393.470684	23.971251
123.408692	3395.175843	23.976269
123.392797	3397.286754	23.981287
123.952671	3399.477899	23.986304
124.040093	3405.486395	23.991322
123.843605	3391.320331	23.996339
123.504606	3397.572382	24.001357
123.940952	3388.196232	24.006375
123.922355	3405.542860	24.011392
124.043403	3426.374242	24.016410
124.753393	3417.526491	24.021427
124.460305	3417.446193	24.026445
124.703844	3413.235487	24.031463
124.511463	3420.136860	24.036480
124.839998	3434.664240	24.041498
125.338067	3431.161690	24.046515
125.125986	3439.843137	24.051533
125.286574	3443.154195	24.056551
125.380065	3441.514103	24.061568
125.074674	3450.008173	24.066586
125.512243	3444.394082	24.071603
125.519422	3469.819952	24.076621
125.587427	3467.855598	24.081639
125.842435	3461.654629	24.086656
125.899581	3474.996767	24.091674
126.228260	3481.759717	24.096691
126.396810	3496.719371	24.101709
126.133881	3489.753653	24.106727
126.841396	3491.000046	24.111744
126.531379	3499.977775	24.116762
126.958280	3511.002112	24.121779
126.833914	3513.107937	24.126797
127.277853	3514.424031	24.131815
127.178011	3511.725304	24.136832
127.218225	3519.388814	24.141850
127.999405	3533.406635	24.146867
127.569599	3544.918716	24.151885
127.869676	3544.982210	24.156903
127.951716	3536.965040	24.161920
128.075442	3544.110471	24.166938
128.440755	3525.065037	24.171955
127.995994	3536.134419	24.176973
128.389519	3555.136802	24.181991
128.483224	3561.409494	24.187008
128.727847	3561.664741	24.192026
128.909139	3553.925549	24.197043
128.725275	3564.303878	24.202061
128.801476	3577.583137	24.207079
129.262697	3583.460535	24.212096
129.318038	3584.168380	24.217114
129.334591	3573.109314	24.222131
129.241705	3593.687183	24.227149
129.645230	3597.398935	24.232167
130.070145	3589.110240	24.237184
130.024157	3587.709771	24.242202
130.354566	3582.263929	24.247219
130.324476	3604.855160	24.252237
130.461606	3599.303873	24.257255
130.971683	3606.013200	24.262272
130.974511	3607.013341	24.267290
131.224427	3601.605354	24.272307
131.204434	3605.070985	24.277325
131.128162	3606.954657	24.282343
131.226237	3604.275409	24.287360
131.145194	3606.080921	24.292378
131.620498	3620.140418	24.297395
131.491782	3630.724773	24.302413
131.829641	3629.835457	24.307431
131.539928	3632.816246	24.312448
131.954428	3634.253745	24.317466
131.607201	3627.648374	24.322483
131.758083	3648.885659	24.327501
132.350825	3648.231009	24.332519
132.195447	3654.855231	24.337536
132.254361	3674.282608	24.342554
132.589462	3676.559504	24.347571
132.696791	3683.802249	24.352589
132.864658	3669.361098	24.357607
133.098643	3688.767375	24.362624
133.259547	3697.018066	24.367642
133.674199	3697.514964	24.372659
133.654871	3695.374888	24.377677
133.662349	3698.618448	24.382695
134.100983	3697.110483	24.387712
134.056654	3694.314654	24.392730
134.370100	3693.523848	24.397747
134.090569	3694.303099	24.402765
134.094226	3700.911892	24.407783
134.433313	3717.240105	24.412800
134.358679	3725.464583	24.417818
134.981063	3720.263339	24.422835
134.730474	3722.363712	24.427853
134.626277	3727.297623	24.432871
135.162610	3726.620245	24.437888
135.149283	3746.677656	24.442906
135.296715	3734.635307	24.447923
135.291822	3740.390089	24.452941
135.683928	3763.972744	24.457959
135.901938	3755.485977	24.462976
135.641499	3766.596060	24.467994
136.065278	3753.768667	24.473011
135.654858	3769.008632	24.478029
135.981968	3785.357720	24.483047
136.186673	3780.395494	24.488064
136.658723	3789.231904	24.493082
137.207459	3797.532352	24.498099
136.845853	3811.328573	24.503117
137.062792	3807.765836	24.508135
137.158695	3801.311921	24.513152
137.131689	3811.107144	24.518170
137.119657	3810.834464	24.523187
137.453636	3830.976436	24.528205
137.505923	3828.607337	24.533223
137.846902	3827.483954	24.538240
137.694507	3835.827980	24.543258
138.116569	3851.022813	24.548275
138.378585	3845.376133	24.553293
138.466805	3854.717753	24.558311
138.674224	3848.394698	24.563328
138.701752	3858.563321	24.568346
138.737826	3869.595451	24.573363
139.076641	3875.583657	24.578381
138.901512	3868.259994	24.583399
138.656492	3874.175537	24.588416
139.285075	3888.668901	24.593434
139.836616	3893.938858	24.598451
139.681872	3888.808815	24.603469
139.966657	3893.202065	24.608487
140.231859	3890.379807	24.613504
140.532003	3914.289544	24.618522
140.456956	3909.225918	24.623539
140.531663	3914.602148	24.628557
140.617978	3915.573444	24.633575
140.914370	3908.298992	24.638592
140.866438	3907.148155	24.643610
141.005627	3905.614491	24.648627
141.245741	3912.782867	24.653645
141.154872	3922.048419	24.658663
141.577526	3927.098695	24.663680
141.221104	3930.939044	24.668698
141.272788	3931.060393	24.673715
141.570524	3923.451150	24.678733
141.627971	3944.965400	24.683751
142.179657	3952.738346	24.688768
141.895637	3953.707692	24.693786
142.130463	3953.497339	24.698803
142.450092	3975.425066	24.703821
142.288037	3983.417160	24.708839
142.599774	3976.667390	24.713856
142.453577	3971.324508	24.718874
142.631777	3990.957638	24.723891
143.046437	4003.237274	24.728909
143.175562	4003.879919	24.733927
142.961503	4007.928395	24.738944
143.283012	4020.326797	24.743962
143.256006	4024.349128	24.748979
143.601425	4028.262613	24.753997
143.751770	4046.959568	24.759015
144.100239	4055.032688	24.764032
144.476439	4056.170054	24.769050
144.223971	4052.598744	24.774067
144.973772	4062.610138	24.779085
144.900578	4075.853197	24.784103
145.245644	4081.332314	24.789120
145.061798	4072.191857	24.794138
144.892546	4065.716261	24.799155
145.679742	4074.260397	24.804173
145.539604	4065.132034	24.809191
145.406325	4075.206030	24.814208
145.669483	4091.663263	24.819226
145.882083	4098.293125	24.824243
145.939533	4097.144705	24.829261
145.800679	4104.473533	24.834279
146.211041	4108.048596	24.839296
146.283934	4126.675701	24.844314
146.510250	4126.397239	24.849331
146.946822	4134.204080	24.854349
146.807279	4142.479950	24.859367
147.309077	4139.330199	24.864384
147.371006	4144.187694	24.869402
146.944560	4150.390574	24.874419
147.625413	4162.578114	24.879437
147.657693	4174.147611	24.884455
147.721354	4164.854700	24.889472
148.000229	4165.701151	24.894490
148.052072	4180.685968	24.899507
148.297427	4186.581603	24.904525
148.059104	4186.347525	24.909543
148.491083	4187.741299	24.914560
148.793957	4201.089666	24.919578
148.894613	4213.147188	24.924595
149.204558	4208.291458	24.929613
148.670497	4211.032857	24.934631
149.203827	4218.578377	24.939648
149.306732	4232.336864	24.944666
149.507872	4230.471514	24.949683
149.940664	4227.468285	24.954701
149.957463	4239.431644	24.959719
150.362771	4247.574856	24.964736
150.407130	4251.876448	24.969754
150.326791	4256.961429	24.974771
150.703396	4249.617458	24.979789
150.822139	4256.713450	24.984807
151.129747	4252.691368	24.989824
151.139510	4264.832606	24.994842
151.045660	4269.790294	24.999859
151.415845	4275.931540	25.004877
151.517397	4283.418475	25.009895
151.620755	4277.461937	25.014912
151.428244	4276.232721	25.019930
151.619671	4290.378249	25.024947
152.173476	4297.819590	25.029965
152.056770	4292.266824	25.034983
152.211624	4294.480503	25.040000
152.193206	4300.777331	25.045018
152.152889	4310.256111	25.050035
152.835499	4307.422055	25.055053
152.471857	4317.109313	25.060071
152.724103	4324.840953	25.065088
153.142901	4338.723635	25.070106
152.989407	4342.614345	25.075123
153.442805	4340.955665	25.080141
153.609313	4361.973546	25.085159
153.344714	4364.041466	25.090176
153.582938	4363.050937	25.095194
153.892654	4380.687959	25.100211
154.366198	4381.068334	25.105229
153.902186	4386.696394	25.110247
154.241578	4392.867756	25.115264
154.920113	4397.985397	25.120282
154.633359	4403.743514	25.125299
154.739021	4401.946764	25.130317
155.428035	4418.817357	25.135335
155.608822	4424.963075	25.140352
155.680487	4424.251153	25.145370
155.993279	4433.605236	25.150387
156.181873	4423.497196	25.155405
156.227498	4429.118025	25.160423
156.351467	4428.760900	25.165440
156.625815	4433.342148	25.170458
156.449835	4449.492888	25.175475
156.779780	4445.707154	25.180493
156.942584	4442.929262	25.185511
156.935195	4449.401174	25.190528
157.236594	4453.754082	25.195546
157.066748	4461.056345	25.200563
157.426692	4474.661115	25.205581
157.054274	4488.415351	25.210599
157.506893	4493.890371	25.215616
157.575517	4507.171499	25.220634
157.517640	4513.502990	25.225651
158.236552	4516.559485	25.230669
157.977414	4528.215897	25.235687
158.256730	4534.197862	25.240704
158.353755	4534.286860	25.245722
158.669757	4555.186851	25.250739
158.802234	4559.623065	25.255757
159.125146	4564.780685	25.260775
159.416390	4575.555472	25.265792
159.491320	4571.522426	25.270810
159.460572	4581.100855	25.275827
159.884548	4579.099552	25.280845
160.168636	4589.225235	25.285863
160.070857	4598.182880	25.290880
160.323957	4597.814991	25.295898
160.318325	4605.688158	25.300915
160.714132	4591.191627	25.305933
160.869374	4613.805584	25.310951
160.793200	4625.944743	25.315968
161.085168	4618.815900	25.320986
160.962430	4626.385462	25.326003
161.129329	4627.609316	25.331021
161.032447	4649.738841	25.336039
161.532127	4646.624058	25.341056
161.831403	4658.445589	25.346074
161.764388	4674.071262	25.351091
162.064302	4670.507985	25.356109
162.212522	4679.161986	25.361127
162.440203	4696.928958	25.366144
162.601232	4700.274900	25.371162
162.657550	4706.105624	25.376179
162.861198	4693.693993	25.381197
162.958822	4716.320261	25.386215
163.245525	4730.201843	25.391232
163.612665	4722.385692	25.396250
163.525836	4728.895401	25.401267
163.568921	4727.840730	25.406285
163.478499	4741.109068	25.411303
163.692823	4745.188446	25.416320
164.229579	4752.165485	25.421338
164.248592	4770.394503	25.426355
164.765872	4766.942354	25.431373
164.692290	4773.254300	25.436391
164.673338	4774.415742	25.441408
165.260006	4787.827403	25.446426
164.944177	4786.926809	25.451443
165.471683	4795.950731	25.456461
165.797090	4799.561338	25.461479
165.915421	4816.692161	25.466496
166.344204	4817.505689	25.471514
166.229586	4815.456166	25.476531
166.407462	4816.327941	25.481549
166.777240	4813.508098	25.486567
166.426639	4813.951311	25.491584
166.849522	4829.131057	25.496602
166.404690	4839.737231	25.501619
166.856279	4835.345248	25.506637
167.103743	4849.258321	25.511655
167.248007	4856.000176	25.516672
167.299228	4852.785164	25.521690
167.262659	4877.424419	25.526707
167.771169	4888.749312	25.531725
167.976077	4893.284738	25.536743
168.129055	4913.598316	25.541760
168.386286	4910.332080	25.546778
168.213129	4921.242958	25.551795
168.549466	4920.322257	25.556813
168.728354	4934.353460	25.561831
168.840912	4936.737984	25.566848
169.224628	4948.382335	25.571866
169.614937	4954.539600	25.576883
169.702744	4961.959525	25.581901
170.006789	4961.703597	25.586919
170.128833	4969.490633	25.591936
170.436503	4978.448076	25.596954
170.310853	4982.849076	25.601971
170.475172	4972.147949	25.606989
170.808997	4982.243964	25.612007
171.161668	4987.573810	25.617024
171.510245	5004.940202	25.622042
171.294785	5009.588862	25.627059
171.829575	4999.805053	25.632077
171.891747	5000.559233	25.637095
172.014065	4984.283909	25.642112
172.000135	4985.662379	25.647130
172.196319	4998.033738	25.652147
172.406315	5006.084787	25.657165
172.661835	5006.253124	25.662183
172.578535	5012.323622	25.667200
172.849637	5006.984502	25.672218
173.115466	5015.184635	25.677236
173.111260	5015.715630	25.682253
173.496056	5019.872530	25.687271
173.443835	5025.572004	25.692288
173.504466	5019.359923	25.697306
173.666465	5030.193108	25.702324
173.439327	5040.664284	25.707341
173.708807	5039.211124	25.712359
173.847233	5061.487365	25.717376
174.169186	5071.181251	25.722394
174.170796	5069.274474	25.727412
174.446065	5075.913817	25.732429
174.833303	5092.510349	25.737447
174.886434	5107.713533	25.742464
175.257649	5100.985597	25.747482
175.487130	5116.038054	25.752500
175.480232	5133.072001	25.757517
175.639927	5129.060274	25.762535
175.650141	5136.243057	25.767552
175.998145	5142.157645	25.772570
176.079511	5148.142416	25.777588
176.098294	5154.219064	25.782605
176.662617	5165.570110	25.787623
176.295925	5179.983692	25.792640
176.829302	5173.908989	25.797658
177.319747	5186.780464	25.802676
177.259854	5197.560126	25.807693
177.461223	5197.219270	25.812711
177.507205	5220.949589	25.817728
177.905507	5220.562098	25.822746
177.962925	5234.034908	25.827764
178.284231	5239.265575	25.832781
178.227947	5251.591430	25.837799
178.036055	5254.200461	25.842816
178.724624	5265.506852	25.847834
178.850200	5278.426083	25.852852
178.919026	5282.768278	25.857869
179.424505	5297.439892	25.862887
179.167207	5303.007437	25.867904
179.495507	5293.824008	25.872922
179.736025	5313.325699	25.877940
179.761315	5320.288388	25.882957
180.107111	5329.565162	25.887975
180.024939	5347.700129	25.892992
180.667184	5344.553427	25.898010
180.521534	5355.375026	25.903028
180.686391	5373.547078	25.908045
180.933187	5372.798213	25.913063
181.077883	5384.256171	25.918080
181.531272	5398.569860	25.923098
181.626930	5405.051221	25.928116
182.044275	5411.920959	25.933133
182.324225	5414.781224	25.938151
182.444674	5426.416621	25.943168
182.813050	5411.497594	25.948186
182.822614	5417.414787	25.953204
182.770011	5425.368269	25.958221
183.318311	5436.519972	25.963239
183.398060	5434.626168	25.968256
183.560342	5440.421589	25.973274
183.429568	5438.377682	25.978292
183.690221	5452.042934	25.983309
183.833693	5461.891255	25.988327
183.843725	5464.093043	25.993344
184.239844	5477.077358	25.998362
184.645008	5495.704318	26.003380
184.430337	5495.968418	26.008397
184.933122	5492.751997	26.013415
184.951811	5511.635230	26.018432
185.083185	5514.465125	26.023450
185.320514	5511.710119	26.028468
185.472638	5522.857651	26.033485
185.821480	5530.341083	26.038503
185.852171	5542.966016	26.043520
186.121230	5532.768998	26.048538
186.680018	5552.470460	26.053556
186.705292	5556.046166	26.058573
186.948212	5556.437449	26.063591
186.628075	5564.508664	26.068608
186.988882	5556.617391	26.073626
186.974331	5576.557061	26.078644
187.300333	5584.182985	26.083661
187.449423	5584.939356	26.088679
187.678649	5603.098395	26.093696
187.880183	5605.873120	26.098714
187.524657	5604.539927	26.103732
187.648078	5618.788687	26.108749
188.561025	5632.762251	26.113767
188.666129	5646.016399	26.118784
188.745255	5646.657467	26.123802
188.900926	5660.124669	26.128820
188.882018	5663.546328	26.133837
189.500349	5673.007863	26.138855
189.628797	5687.682038	26.143872
189.508662	5686.375096	26.148890
189.919999	5696.528813	26.153908
190.027924	5710.129799	26.158925
190.154599	5705.261349	26.163943
190.445810	5727.744906	26.168960
190.908113	5728.979379	26.173978
191.021378	5735.322363	26.178996
191.088073	5746.713852	26.184013
191.699131	5753.632289	26.189031
191.568400	5766.670937	26.194048
191.488424	5770.569372	26.199066
191.893660	5779.249922	26.204084
191.868255	5788.610338	26.209101
192.281124	5783.308761	26.214119
192.449145	5803.939799	26.219136
192.614409	5800.365833	26.224154
192.679971	5807.183504	26.229172
193.126186	5821.789066	26.234189
193.356977	5819.085546	26.239207
193.798764	5818.176693	26.244224
193.683254	5831.989548	26.249242
193.747704	5842.099832	26.254260
193.999105	5846.072637	26.259277
194.484314	5842.994648	26.264295
194.259234	5864.479667	26.269312
194.624524	5866.682670	26.274330
194.466061	5881.086278	26.279348
194.911179	5887.418364	26.284365
195.335384	5881.268989	26.289383
195.595923	5905.029718	26.294400
195.646847	5912.045437	26.299418
196.183469	5917.978081	26.304436
196.209747	5906.291046	26.309453
196.568236	5921.248197	26.314471
196.536376	5926.411279	26.319488
196.569905	5933.363440	26.324506
196.843543	5935.208319	26.329524
196.932122	5950.517136	26.334541
197.392359	5949.075059	26.339559
197.138985	5952.947033	26.344576
197.640887	5960.116247	26.349594
197.970936	5970.806867	26.354612
197.736464	5978.138798	26.359629
198.359569	5993.720622	26.364647
198.375864	6003.497614	26.369664
198.298190	6009.412882	26.374682
198.734014	6008.905858	26.379700
198.803738	6032.207354	26.384717
199.375517	6028.995817	26.389735
199.416296	6043.261012	26.394752
199.387349	6054.569817	26.399770
199.815679	6054.944693	26.404788
199.686080	6054.163223	26.409805
199.742650	6065.070361	26.414823
200.173388	6083.936985	26.419840
200.199014	6076.334754	26.424858
200.569060	6094.065004	26.429876
200.797461	6102.574538	26.434893
201.061830	6103.937905	26.439911
201.300576	6120.198771	26.444928
201.700642	6119.804675	26.449946
202.110377	6130.435554	26.454964
201.893685	6145.391452	26.459981
202.375079	6140.574646	26.464999
202.501222	6160.092005	26.470016
202.515386	6154.032029	26.475034
202.971388	6143.979007	26.480052
202.952824	6168.948641	26.485069
203.068100	6175.348285	26.490087
203.388879	6177.012182	26.495104
203.217103	6190.872002	26.500122
203.563256	6191.824814	26.505140
203.499260	6203.738985	26.510157
204.115795	6208.762688	26.515175
204.404068	6231.821855	26.520192
204.384203	6236.942107	26.525210
204.651506	6236.082668	26.530228
204.852897	6248.371984	26.535245
204.803082	6258.011102	26.540263
204.992654	6270.845248	26.545280
205.268877	6287.428695	26.550298
205.958817	6298.757616	26.555316
205.736557	6301.321043	26.560333
206.209375	6315.171522	26.565351
206.646967	6314.159131	26.570368
206.947204	6326.126808	26.575386
207.336458	6329.633018	26.580404
207.363340	6355.015638	26.585421
207.367056	6349.538082	26.590439
207.574510	6350.136974	26.595456
207.788682	6364.028009	26.600474
207.989353	6360.871396	26.605492
208.101938	6360.897990	26.610509
208.445344	6373.992220	26.615527
208.599740	6387.475942	26.620544
208.753819	6386.198597	26.625562
209.068193	6399.196376	26.630580
209.243122	6415.451718	26.635597
209.666479	6420.471019	26.640615
209.534773	6420.040267	26.645632
209.776279	6441.279243	26.650650
209.993404	6449.699160	26.655668
210.000583	6447.772426	26.660685
210.477101	6463.440752	26.665703
210.730869	6467.429107	26.670720
210.890071	6469.809683	26.675738
211.036218	6481.192339	26.680756
211.134638	6496.935710	26.685773
211.544078	6496.224459	26.690791
211.732029	6509.106379	26.695808
211.776622	6517.673314	26.700826
212.180797	6514.023901	26.705844
212.335843	6527.283491	26.710861
212.228192	6528.136946	26.715879
212.837296	6539.740696	26.720896
212.592702	6553.381750	26.725914
213.184580	6560.735986	26.730932
213.507232	6570.234840	26.735949
213.798620	6574.690848	26.740967
213.795438	6579.587605	26.745984
214.065035	6583.791326	26.751002
214.216716	6591.808017	26.756020
214.397979	6606.098994	26.761037
214.224833	6611.773709	26.766055
214.449087	6620.912343	26.771072
214.686806	6630.279320	26.776090
215.003297	6643.340078	26.781108
215.299536	6653.281913	26.786125
215.456747	6660.720067	26.791143
215.690936	6674.156776	26.796160
215.714707	6682.244054	26.801178
216.114456	6700.506901	26.806196
216.257284	6709.768824	26.811213
216.533003	6717.343122	26.816231
216.816538	6720.834402	26.821248
217.036789	6745.044492	26.826266
217.042669	6749.778876	26.831284
217.014288	6763.802918	26.836301
217.296267	6778.747504	26.841319
217.816991	6785.803607	26.846336
218.090587	6814.096713	26.851354
218.753938	6820.104507	26.856372
218.560915	6826.391676	26.861389
218.874877	6836.397128	26.866407
219.172156	6838.497258	26.871424
218.930134	6854.676249	26.876442
220.041452	6851.575776	26.881460
219.901728	6859.041588	26.886477
220.028903	6867.109591	26.891495
220.382605	6877.190918	26.896512
220.759579	6885.851171	26.901530
220.862446	6894.636447	26.906548
221.099693	6907.315198	26.911565
221.206279	6911.443512	26.916583
221.417856	6922.857232	26.921600
221.647590	6935.167825	26.926618
221.651399	6938.273633	26.931636
222.081616	6953.150943	26.936653
222.220085	6952.961972	26.941671
222.489769	6964.499204	26.946688
222.424475	6974.077984	26.951706
223.027241	6980.032185	26.956724
223.414324	6997.141893	26.961741
223.379416	7016.518077	26.966759
223.783660	7016.843084	26.971776
223.776268	7019.467655	26.976794
224.282589	7041.893874	26.981812
224.598811	7038.201314	26.986829
224.402688	7040.839670	26.991847
224.875852	7043.186921	26.996864
225.166463	7058.000950	27.001882
225.379235	7066.178751	27.006900
225.508942	7075.607074	27.011917
225.379500	7087.307930	27.016935
225.816548	7085.118060	27.021952
226.276212	7095.012435	27.026970
226.432065	7103.047637	27.031988
226.681136	7113.480119	27.037005
226.940616	7132.605109	27.042023
227.141697	7122.468371	27.047040
227.111916	7143.993743	27.052058
227.556878	7146.301230	27.057076
228.142690	7148.558239	27.062093
228.017443	7155.286341	27.067111
228.576665	7157.048724	27.072128
228.785805	7178.486198	27.077146
228.748361	7174.492282	27.082164
229.298380	7172.849793	27.087181
229.072485	7182.201287	27.092199
229.425034	7191.414816	27.097216
229.569833	7197.396635	27.102234
229.589914	7200.891396	27.107252
229.811215	7209.771919	27.112269
230.060207	7215.664813	27.117287
230.082039	7225.709928	27.122304
230.094438	7243.926663	27.127322
230.640087	7257.876941	27.132340
230.848134	7266.535426	27.137357
230.721636	7281.749613	27.142375
231.327486	7286.721625	27.147392
231.501968	7306.482029	27.152410
231.811045	7309.833673	27.157428
232.250355	7319.617709	27.162445
231.957598	7336.079723	27.167463
232.778877	7338.135709	27.172480
232.762671	7349.620105	27.177498
232.885239	7357.297584	27.182516
233.254265	7367.360996	27.187533
233.534435	7392.175002	27.192551
233.848543	7391.674386	27.197568
234.173925	7410.328427	27.202586
234.064420	7420.637308	27.207604
234.718884	7423.786490	27.212621
234.563041	7440.372370	27.217639
235.340524	7438.937312	27.222656
235.053168	7458.918606	27.227674
235.521676	7473.837695	27.232692
235.792640	7470.448894	27.237709
235.875476	7484.667580	27.242727
236.116196	7497.497730	27.247744
236.617683	7512.976783	27.252762
236.612233	7522.410724	27.257780
237.035955	7528.317386	27.262797
237.123781	7545.174572	27.267815
237.378386	7555.047652	27.272832
237.643679	7555.520717	27.277850
237.826146	7574.506696	27.282868
238.253279	7579.585711	27.287885
238.244628	7596.918978	27.292903
238.301423	7605.904388	27.297920
238.738947	7622.283826	27.302938
238.920940	7633.664739	27.307956
239.193583	7639.333074	27.312973
239.445859	7650.017918	27.317991
239.727573	7664.492875	27.323008
239.932176	7682.411588	27.328026
240.276970	7690.067021	27.333044
240.825627	7708.326488	27.338061
240.691552	7721.786927	27.343079
241.055249	7717.089179	27.348096
241.316307	7736.309261	27.353114
241.423574	7745.084783	27.358132
241.823872	7746.748999	27.363149
242.051991	7762.766739	27.368167
242.296492	7762.917894	27.373184
242.257597	7773.582126	27.378202
242.327089	7789.043846	27.383220
243.112711	7806.256041	27.388237
243.198182	7812.430462	27.393255
243.222932	7834.607917	27.398272
243.568887	7840.807839	27.403290
243.619623	7852.076854	27.408308
244.255072	7862.095645	27.413325
244.418054	7869.164013	27.418343
244.724222	7875.594330	27.423360
244.908878	7882.946598	27.428378
245.403576	7892.160310	27.433396
245.677838	7895.463847	27.438413
245.408998	7920.942309	27.443431
245.732335	7917.422098	27.448448
246.042610	7916.499026	27.453466
246.254703	7941.052930	27.458484
246.648782	7942.127770	27.463501
246.790790	7961.205727	27.468519
246.907824	7958.368180	27.473536
247.087550	7981.143472	27.478554
247.284565	7989.658801	27.483572
247.664066	7993.801433	27.488589
247.624668	8014.025461	27.493607
248.136526	8011.176568	27.498624
248.305051	8037.322271	27.503642
248.460223	8049.964155	27.508660
249.024182	8066.542021	27.513677
249.234357	8078.256600	27.518695
249.747749	8087.963143	27.523712
249.648917	8099.795599	27.528730
250.017669	8108.549275	27.533748
250.468538	8120.538727	27.538765
250.410189	8130.325386	27.543783
250.705115	8138.086688	27.548800
251.020503	8153.046102	27.553818
250.923324	8158.576793	27.558836
251.482614	8168.680296	27.563853
251.410054	8181.436873	27.568871
251.860985	8184.539146	27.573888
252.279371	8208.246559	27.578906
252.410431	8225.915282	27.583924
252.434378	8240.933051	27.588941
252.403330	8250.443986	27.593959
252.823173	8259.903235	27.598976
253.426592	8283.139764	27.603994
253.382759	8305.173828	27.609012
254.245966	8311.681206	27.614029
254.202118	8332.247247	27.619047
254.775446	8341.884551	27.624064
255.027689	8361.877003	27.629082
254.816082	8369.326269	27.634100
255.468799	8380.390804	27.639117
255.848885	8389.171252	27.644135
255.897702	8396.797575	27.649152
256.306277	8405.709325	27.654170
256.207555	8424.159316	27.659188
256.740851	8428.318997	27.664205
256.993605	8445.583696	27.669223
257.423026	8453.232505	27.674240
257.794901	8463.684401	27.679258
257.728047	8479.354329	27.684276
258.075089	8479.584143	27.689293
257.892405	8496.342502	27.694311
258.128279	8510.152832	27.699328
258.674213	8530.326773	27.704346
259.051208	8538.457403	27.709364
259.540572	8537.881949	27.714381
259.531996	8552.497792	27.719399
260.014664	8569.593990	27.724416
260.249235	8568.262845	27.729434
260.434609	8577.414858	27.734452
261.175307	8573.402928	27.739469
260.896815	8585.847913	27.744487
261.302106	8600.493676	27.749504
261.660635	8598.082304	27.754522
261.374174	8617.477474	27.759540
261.950802	8622.912221	27.764557
261.882676	8641.124005	27.769575
262.152221	8649.205216	27.774592
262.547245	8649.525388	27.779610
262.568539	8669.210219	27.784628
263.141675	8679.068733	27.789645
263.581579	8689.093352	27.794663
263.327692	8698.522610	27.799680
263.795660	8705.467750	27.804698
263.885786	8723.740068	27.809716
264.480214	8733.374272	27.814733
264.503231	8738.276969	27.819751
264.867238	8760.857024	27.824768
264.984835	8767.396123	27.829786
265.388783	8794.371087	27.834804
265.463532	8792.278822	27.839821
266.079850	8812.044239	27.844839
266.298916	8824.626129	27.849856
266.568532	8840.278383	27.854874
266.666766	8843.407606	27.859892
267.281104	8853.237658	27.864909
267.519687	8866.359559	27.869927
267.854984	8860.169458	27.874944
268.147795	8880.557081	27.879962
268.430005	8893.485892	27.884980
268.754132	8899.585404	27.889997
268.884018	8907.218181	27.895015
268.915045	8911.504013	27.900032
269.362639	8924.785804	27.905050
269.512800	8930.802076	27.910068
269.850830	8943.965284	27.915085
270.438758	8952.306161	27.920103
270.325613	8957.236560	27.925120
270.985159	8975.925083	27.930138
270.880934	8977.987329	27.935156
271.165827	8996.254663	27.940173
271.403622	9002.405621	27.945191
271.560794	9017.289488	27.950208
271.955140	9026.279541	27.955226
271.905315	9047.668193	27.960244
272.368132	9067.098005	27.965261
272.675503	9074.636746	27.970279
272.651188	9085.649903	27.975296
273.327914	9097.803517	27.980314
273.099108	9116.081982	27.985332
273.909126	9123.905087	27.990349
273.934842	9139.456882	27.995367
274.335504	9158.069325	28.000384
274.525691	9173.453307	28.005402
274.961521	9194.462953	28.010420
275.482914	9206.489424	28.015437
275.694511	9219.486354	28.020455
275.576368	9230.340645	28.025472
276.482965	9227.492882	28.030490
276.987377	9253.811852	28.035508
277.383861	9256.193509	28.040525
277.163751	9255.145080	28.045543
277.603168	9266.638223	28.050560
278.206893	9269.530469	28.055578
278.326120	9282.879743	28.060596
278.214294	9270.189252	28.065613
278.735222	9284.233347	28.070631
278.851558	9312.779087	28.075648
279.002397	9306.330422	28.080666
279.237186	9338.835823	28.085684
279.561804	9337.572609	28.090701
279.804359	9351.767710	28.095719
279.539743	9357.795422	28.100736
280.512767	9369.732308	28.105754
280.907492	9380.354796	28.110772
281.038631	9383.573674	28.115789
281.060661	9389.386000	28.120807
281.336383	9413.189925	28.125824
281.834085	9412.524738	28.130842
281.697482	9425.424808	28.135860
281.970097	9438.544941	28.140877
282.443518	9452.858662	28.145895
282.596177	9469.729546	28.150912
282.699403	9475.298696	28.155930
282.928373	9488.435173	28.160948
283.265241	9515.308031	28.165965
283.407873	9525.493337	28.170983
283.301253	9553.938609	28.176000
284.257834	9562.862951	28.181018
284.395861	9574.131968	28.186036
284.670286	9601.608311	28.191053
285.254390	9607.635760	28.196071
285.311798	9619.703610	28.201088
285.518194	9639.916165	28.206106
285.789966	9658.369332	28.211124
286.036836	9673.362811	28.216141
286.315307	9683.770041	28.221159
286.479033	9717.660682	28.226176
287.192043	9732.647493	28.231194
287.247518	9743.875869	28.236212
287.785734	9770.458652	28.241229
288.217641	9780.762967	28.246247
288.490751	9796.336546	28.251264
289.135297	9801.940976	28.256282
289.154498	9818.975165	28.261300
289.345469	9816.564628	28.266317
289.841111	9828.832342	28.271335
289.900068	9836.735517	28.276352
290.227370	9850.251518	28.281370
290.857659	9861.705660	28.286388
290.772985	9872.779255	28.291405
291.087028	9895.485341	28.296423
291.220270	9910.986206	28.301440
292.000949	9915.391641	28.306458
291.994840	9932.344649	28.311476
292.177300	9942.470269	28.316493
292.910539	9945.708593	28.321511
293.002043	9963.609343	28.326528
293.388384	9973.936689	28.331546
293.582371	9990.533193	28.336564
294.353867	9998.987873	28.341581
294.197000	9995.280435	28.346599
294.474717	10018.983786	28.351616
294.583230	10018.913148	28.356634
295.051666	10044.117996	28.361652
295.298970	10054.416649	28.366669
295.661081	10075.347276	28.371687
295.661263	10093.625558	28.376704
295.804483	10099.873789	28.381722
296.385611	10124.328572	28.386740
296.810680	10137.226399	28.391757
296.662217	10149.222647	28.396775
297.124238	10168.012779	28.401792
297.612365	10179.306256	28.406810
297.879724	10202.130540	28.411828
297.818841	10215.461335	28.416845
298.593965	10216.482942	28.421863
298.274701	10247.251721	28.426880
298.610228	10258.894368	28.431898
299.017480	10276.199718	28.436916
299.289653	10290.896088	28.441933
299.478133	10306.325480	28.446951
299.810927	10322.366926	28.451968
300.584431	10335.844958	28.456986
301.037114	10355.574508	28.462004
301.347219	10364.584724	28.467021
301.695115	10370.112657	28.472039
301.533863	10387.355607	28.477056
301.849318	10397.435381	28.482074
302.351429	10404.959947	28.487092
302.503867	10417.600716	28.492109
302.921219	10431.409308	28.497127
303.026854	10446.946518	28.502144
303.465160	10455.434657	28.507162
303.964198	10474.677135	28.512180
304.037154	10487.753505	28.517197
304.893874	10489.299119	28.522215
304.975507	10499.140875	28.527232
305.473595	10505.529417	28.532250
305.848363	10509.957535	28.537268
306.112942	10532.375343	28.542285
306.476037	10535.333904	28.547303
306.551730	10535.877802	28.552320
307.079232	10550.625948	28.557338
307.007331	10568.871782	28.562356
307.256442	10574.519448	28.567373
307.521506	10580.780329	28.572391
307.853393	10604.014943	28.577408
308.162128	10620.707703	28.582426
308.732439	10628.793186	28.587444
308.663644	10648.314243	28.592461
309.100402	10656.714306	28.597479
309.126916	10675.175325	28.602496
309.409214	10686.340321	28.607514
309.676651	10694.280667	28.612532
309.868862	10727.941340	28.617549
310.568858	10736.827511	28.622567
310.731561	10753.982161	28.627584
311.215470	10771.642237	28.632602
311.475113	10786.404112	28.637620
311.856198	10813.739232	28.642637
312.160289	10821.977015	28.647655
312.215329	10836.872021	28.652672
312.766952	10850.906180	28.657690
312.769243	10867.536650	28.662708
313.133504	10892.793698	28.667725
313.777657	10909.408914	28.672743
313.778285	10928.935176	28.677760
314.344197	10945.423748	28.682778
314.800404	10952.396839	28.687796
314.969739	10971.486236	28.692813
315.280489	10992.732221	28.697831
315.498934	11014.160042	28.702848
316.018232	11031.887445	28.707866
316.124379	11048.981759	28.712884
315.974172	11062.298730	28.717901
317.105368	11083.053178	28.722919
317.435620	11102.531144	28.727936
317.472659	11110.214103	28.732954
317.842900	11134.655883	28.737972
318.021636	11139.443249	28.742989
318.494813	11150.149189	28.748007
318.701085	11173.252623	28.753024
319.029501	11192.342586	28.758042
319.305839	11201.121676	28.763060
319.846815	11229.644878	28.768077
320.304196	11237.505180	28.773095
320.445091	11252.292339	28.778112
320.516003	11273.749882	28.783130
321.033657	11280.242986	28.788148
320.948829	11301.226053	28.793165
321.294161	11310.455399	28.798183
321.597440	11332.972306	28.803200
321.792026	11352.067607	28.808218
322.419492	11363.175781	28.813236
322.596461	11384.771561	28.818253
323.316547	11395.293713	28.823271
323.356801	11404.466693	28.828288
323.757984	11427.599905	28.833306
324.278807	11447.029432	28.838324
324.288385	11464.063467	28.843341
324.679652	11479.645205	28.848359
325.068697	11497.532390	28.853376
325.351580	11518.274955	28.858394
325.844565	11522.353244	28.863412
325.761101	11544.242616	28.868429
326.133026	11557.219220	28.873447
326.385155	11579.346569	28.878464
326.749183	11599.347092	28.883482
327.548788	11610.485287	28.888500
327.885886	11635.564446	28.893517
328.058524	11649.358593	28.898535
328.317913	11661.891877	28.903552
328.868550	11680.132846	28.908570
329.388734	11693.379985	28.913588
329.340652	11720.461571	28.918605
329.712892	11724.691442	28.923623
330.009609	11750.945427	28.928640
330.030203	11763.279357	28.933658
330.924594	11789.215577	28.938676
331.010821	11807.226277	28.943693
331.454124	11825.323158	28.948711
331.783583	11844.940960	28.953728
331.916389	11863.086514	28.958746
332.556592	11869.541682	28.963764
332.910359	11893.399697	28.968781
333.259272	11899.148967	28.973799
333.840296	11912.064644	28.978816
333.791629	11933.895336	28.983834
334.359124	11950.548749	28.988852
334.490427	11964.643272	28.993869
335.180415	11970.190723	28.998887
335.611363	11989.265437	29.003904
335.548788	12001.893590	29.008922
335.838811	12018.871567	29.013940
336.002662	12044.047880	29.018957
336.257201	12062.026144	29.023975
337.037957	12076.063225	29.028992
337.308701	12085.172013	29.034010
337.862409	12107.593780	29.039028
338.037449	12127.299221	29.044045
338.447992	12140.551221	29.049063
338.556083	12150.576007	29.054080
338.755279	12167.334671	29.059098
338.879120	12186.943988	29.064116
339.200604	12203.494062	29.069133
339.669840	12220.690455	29.074151
340.664158	12244.369633	29.079168
340.640185	12255.968789	29.084186
341.173660	12272.229937	29.089204
341.245981	12295.592568	29.094221
341.670390	12309.799325	29.099239
342.402725	12323.575765	29.104256
342.250128	12342.701195	29.109274
342.649239	12370.275752	29.114292
342.887282	12374.615210	29.119309
343.496631	12390.855103	29.124327
344.044091	12403.770061	29.129344
343.942207	12415.195209	29.134362
344.159905	12426.203998	29.139380
344.321899	12441.200360	29.144397
344.443054	12461.053534	29.149415
345.081890	12467.547019	29.154432
345.393229	12500.342754	29.159450
345.667367	12512.103787	29.164468
346.524117	12529.157657	29.169485
346.659842	12558.393712	29.174503
346.963533	12564.762890	29.179520
347.163488	12590.294271	29.184538
347.345105	12603.711928	29.189556
347.934117	12612.720592	29.194573
348.441385	12631.364010	29.199591
348.845585	12652.423554	29.204608
348.834673	12686.902698	29.209626
349.600179	12690.458564	29.214644
349.618195	12707.312404	29.219661
349.813749	12726.671051	29.224679
350.771474	12740.829331	29.229696
351.083881	12763.804411	29.234714
351.081738	12788.663512	29.239732
351.288542	12801.789999	29.244749
351.430688	12814.550837	29.249767
352.091011	12837.395719	29.254784
352.076269	12863.700043	29.259802
352.760287	12886.664430	29.264820
353.234024	12906.699685	29.269837
353.562907	12933.967121	29.274855
353.919197	12947.294504	29.279872
354.279704	12969.738089	29.284890
354.837953	12987.246503	29.289908
355.280269	13011.496275	29.294925
355.280271	13026.287950	29.299943
356.051017	13040.387324	29.304960
356.069915	13059.543456	29.309978
356.367056	13069.842278	29.314996
357.146330	13098.138355	29.320013
357.520429	13115.451522	29.325031
357.661794	13131.926415	29.330048
358.013927	13154.226267	29.335066
358.375442	13173.385689	29.340084
358.604326	13187.307943	29.345101
358.937193	13212.405654	29.350119
359.417964	13237.448651	29.355136
359.552286	13256.669009	29.360154
359.882944	13279.553435	29.365172
360.547798	13300.244446	29.370189
360.782668	13309.476290	29.375207
360.901805	13326.968539	29.380224
361.423164	13359.016009	29.385242
361.974766	13369.530931	29.390260
362.429272	13395.329847	29.395277
362.854712	13420.198592	29.400295
363.056203	13428.782022	29.405312
363.205248	13452.803555	29.410330
363.997344	13471.349502	29.415348
364.284903	13482.003744	29.420365
364.614015	13510.352005	29.425383
365.140382	13527.054312	29.430400
365.414620	13543.594015	29.435418
366.084637	13558.492739	29.440436
366.272958	13576.517556	29.445453
366.550242	13596.600106	29.450471
367.057266	13604.488366	29.455488
366.908553	13630.789475	29.460506
367.522799	13650.661399	29.465524
368.026384	13665.434693	29.470541
368.241029	13670.621307	29.475559
368.724977	13675.661524	29.480576
368.862224	13693.754455	29.485594
368.895428	13713.837465	29.490612
369.627399	13724.273804	29.495629
369.593770	13741.910369	29.500647
370.186706	13755.624431	29.505664
370.169728	13787.469571	29.510682
370.611504	13799.603060	29.515700
370.968319	13829.709644	29.520717
371.729094	13852.751611	29.525735
371.956598	13868.184127	29.530752
372.147508	13894.097648	29.535770
372.690353	13926.467993	29.540788
372.940978	13939.534719	29.545805
373.088845	13969.781629	29.550823
374.213451	13978.508097	29.555840
374.406645	14008.204780	29.560858
374.626860	14022.384810	29.565876
375.544517	14048.228917	29.570893
375.821107	14067.374124	29.575911
376.080665	14069.859969	29.580928
376.292183	14099.724462	29.585946
376.716338	14120.163530	29.590964
377.171265	14129.784490	29.595981
377.253474	14145.603171	29.600999
378.072034	14168.699633	29.606016
377.974774	14192.883848	29.611034
378.696039	14205.968622	29.616052
379.013420	14218.020806	29.621069
379.291888	14246.476001	29.626087
380.053336	14270.806880	29.631104
380.357855	14289.111036	29.636122
380.836314	14310.542927	29.641140
381.139465	14327.947269	29.646157
381.446019	14344.113108	29.651175
381.845270	14352.956528	29.656192
381.764223	14387.304472	29.661210
382.515036	14402.747039	29.666228
382.907245	14424.609443	29.671245
383.251558	14437.390236	29.676263
383.740194	14449.185197	29.681280
383.973495	14478.737374	29.686298
384.221050	14494.764150	29.691316
384.911508	14526.701837	29.696333
385.114546	14544.441033	29.701351
385.590105	14567.629606	29.706368
386.202886	14579.853662	29.711386
386.653012	14597.408928	29.716404
386.992611	14613.209788	29.721421
387.226379	14633.060229	29.726439
387.908332	14643.934425	29.731456
388.028598	14659.419122	29.736474
388.842633	14678.815528	29.741492
389.195089	14691.598375	29.746509
389.313328	14710.282673	29.751527
389.722185	14719.424788	29.756544
389.823493	14746.073572	29.761562
390.117565	14770.108792	29.766580
390.717480	14779.840016	29.771597
390.929634	14815.102896	29.776615
391.397873	14839.692032	29.781632
391.259555	14854.159391	29.786650
391.967756	14879.986911	29.791668
392.466710	14895.162983	29.796685
392.658208	14919.302888	29.801703
393.152799	14943.209013	29.806720
393.549825	14968.324261	29.811738
393.710680	14988.682335	29.816756
394.382338	15005.637955	29.821773
394.664726	15030.152226	29.826791
395.202255	15042.252564	29.831808
395.603740	15060.384360	29.836826
395.850960	15067.053789	29.841844
396.642901	15085.970860	29.846861
396.773175	15120.407034	29.851879
397.072909	15131.856177	29.856896
397.556800	15142.294261	29.861914
397.902759	15170.888703	29.866932
398.202964	15183.752706	29.871949
398.681599	15220.976935	29.876967
399.227418	15234.500478	29.881984
399.192818	15253.000800	29.887002
399.622234	15281.430738	29.892020
400.365083	15299.243996	29.897037
400.580469	15325.285119	29.902055
401.260516	15344.346306	29.907072
401.460069	15373.586167	29.912090
401.797798	15396.393076	29.917108
402.438191	15400.802859	29.922125
402.879757	15431.918833	29.927143
403.559998	15448.254475	29.932160
403.696772	15468.203093	29.937178
404.379245	15490.570801	29.942196
404.530263	15510.930972	29.947213
404.794024	15529.492211	29.952231
405.430543	15553.657960	29.957248
405.912223	15573.697947	29.962266
405.811078	15598.566747	29.967284
406.429453	15606.368921	29.972301
407.306539	15632.966909	29.977319
407.311686	15655.453537	29.982336
407.695054	15674.981586	29.987354
407.929246	15694.251927	29.992372
408.737107	15723.172797	29.997389
409.153931	15733.804897	30.002407
409.896189	15759.726184	30.007424
410.119308	15769.895940	30.012442
410.578633	15793.786546	30.017460
411.137382	15800.783281	30.022477
411.242950	15830.066986	30.027495
412.000230	15837.092646	30.032512
412.444063	15854.087866	30.037530
412.790270	15876.246552	30.042548
412.919889	15897.248479	30.047565
413.380206	15914.459099	30.052583
413.759056	15935.984222	30.057600
414.179494	15949.256291	30.062618
414.340103	15977.637775	30.067636
414.940534	15990.344751	30.072653
415.166419	16004.196893	30.077671
415.711009	16042.751552	30.082688
415.630414	16059.690128	30.087706
416.119238	16090.540781	30.092724
416.712632	16112.837894	30.097741
417.358730	16141.260437	30.102759
417.637567	16151.756462	30.107776
418.256919	16179.302050	30.112794
418.481424	16198.065908	30.117812
419.169178	16217.685804	30.122829
419.199519	16249.938229	30.127847
419.688187	16273.202624	30.132864
420.263394	16293.790919	30.137882
420.264908	16316.266256	30.142900
421.253446	16342.512979	30.147917
421.377722	16366.292540	30.152935
421.672838	16387.698630	30.157952
422.321706	16399.482338	30.162970
422.300631	16423.679544	30.167988
423.180970	16439.640420	30.173005
423.254889	16451.744785	30.178023
423.810395	16479.003907	30.183040
424.462656	16491.725209	30.188058
424.689260	16521.932237	30.193076
425.375101	16537.074027	30.198093
425.564677	16562.558661	30.203111
425.896489	16581.233440	30.208128
426.529359	16594.858019	30.213146
426.615969	16622.260277	30.218164
427.159834	16650.342677	30.223181
427.487187	16676.440741	30.228199
427.858866	16698.877495	30.233216
428.563618	16719.894466	30.238234
428.916916	16750.410495	30.243252
429.339117	16771.572852	30.248269
429.881294	16801.762476	30.253287
429.985644	16828.369456	30.258304
430.463403	16843.964166	30.263322
430.838603	16874.998120	30.268340
431.376351	16891.148853	30.273357
432.044734	16922.844477	30.278375
432.570043	16952.105205	30.283392
433.294271	16975.093504	30.288410
432.950337	17002.535312	30.293428
433.913051	17017.621480	30.298445
434.035919	17045.732496	30.303463
434.190506	17071.848682	30.308480
435.104865	17092.242576	30.313498
435.469281	17114.036601	30.318516
435.669083	17152.489562	30.323533
436.268433	17181.410548	30.328551
436.871824	17202.680819	30.333568
437.541127	17230.434875	30.338586
437.992951	17258.115643	30.343604
438.612571	17276.913424	30.348621
439.002609	17298.432004	30.353639
439.431548	17322.648291	30.358656
439.784240	17333.010208	30.363674
440.308574	17355.486989	30.368692
440.571224	17373.589025	30.373709
441.334620	17395.807304	30.378727
441.635866	17419.146663	30.383744
441.886106	17445.159929	30.388762
442.128658	17460.858313	30.393780
442.645253	17476.987582	30.398797
443.040879	17508.114115	30.403815
443.710510	17535.040993	30.408832
443.793814	17558.155647	30.413850
444.089285	17596.051217	30.418868
444.817785	17615.937806	30.423885
445.563601	17643.162452	30.428903
445.693855	17667.223800	30.433920
445.971759	17689.518462	30.438938
446.583435	17725.968623	30.443956
446.951284	17747.579622	30.448973
447.466210	17770.285786	30.453991
447.865024	17796.769009	30.459008
448.422626	17815.273795	30.464026
448.597502	17844.729749	30.469044
449.055596	17872.985300	30.474061
449.505625	17892.751540	30.479079
450.249305	17931.992666	30.484096
450.885927	17955.836077	30.489114
451.138739	17975.658561	30.494132
451.589105	18006.322465	30.499149
452.143794	18020.184572	30.504167
452.353372	18053.040520	30.509184
453.012091	18064.176169	30.514202
453.388122	18082.937080	30.519220
453.597257	18108.117450	30.524237
454.200302	18124.625405	30.529255
454.434106	18152.069949	30.534272
454.886940	18170.534628	30.539290
455.554594	18200.431974	30.544308
456.224757	18218.249859	30.549325
456.590921	18239.842720	30.554343
456.857723	18271.527648	30.559360
457.374815	18283.532158	30.564378
457.472447	18318.042334	30.569396
458.133817	18348.319946	30.574413
458.860124	18367.778061	30.579431
459.148698	18395.966163	30.584448
459.668011	18427.093753	30.589466
459.865156	18455.713224	30.594484
460.031578	18477.691421	30.599501
460.849221	18506.984528	30.604519
461.027306	18531.544866	30.609536
461.483541	18562.082378	30.614554
462.393178	18603.105715	30.619572
462.841554	18618.532728	30.624589
463.484266	18635.420284	30.629607
463.792549	18676.234717	30.634624
464.848057	18705.396103	30.639642
465.157057	18728.293586	30.644660
465.700057	18733.066879	30.649677
466.126231	18760.153632	30.654695
466.721226	18784.705850	30.659712
466.794367	18808.253188	30.664730
467.341221	18830.380682	30.669748
468.221688	18842.650828	30.674765
468.713356	18861.027952	30.679783
469.163636	18882.741026	30.684800
469.896018	18890.991043	30.689818
470.223424	18918.207207	30.694836
470.553716	18928.946237	30.699853
471.297992	18950.891320	30.704871
471.682670	18975.344048	30.709888
472.063249	18991.293717	30.714906
472.439021	19016.859821	30.719924
472.705546	19032.442003	30.724941
473.171866	19065.992314	30.729959
473.665371	19090.143839	30.734976
473.813384	19108.492892	30.739994
474.341195	19139.196999	30.745012
474.921418	19167.220500	30.750029
475.358327	19188.297909	30.755047
475.472002	19214.297029	30.760064
475.832476	19235.569679	30.765082
476.594903	19265.794988	30.770100
477.057387	19303.610869	30.775117
477.586225	19329.064958	30.780135
477.720491	19357.784054	30.785152
478.448589	19385.588854	30.790170
478.784789	19422.015852	30.795188
479.178693	19447.105836	30.800205
480.058241	19482.095807	30.805223
480.534645	19511.576555	30.810240
481.083458	19548.924498	30.815258
481.541259	19567.648765	30.820276
481.770973	19600.131410	30.825293
482.132953	19630.407370	30.830311
482.442942	19662.094115	30.835328
482.880901	19678.964106	30.840346
483.665118	19711.922389	30.845364
484.062656	19743.898819	30.850381
484.597477	19755.288617	30.855399
484.929690	19784.078424	30.860416
485.163562	19816.819817	30.865434
485.797527	19854.350867	30.870452
485.812099	19884.340459	30.875469
486.501971	19915.209946	30.880487
487.166997	19954.871834	30.885504
487.670398	19975.579548	30.890522
487.834331	20016.293031	30.895540
488.474676	20046.007951	30.900557
489.598349	20074.889038	30.905575
489.653791	20105.371699	30.910592
490.704262	20133.120755	30.915610
491.316385	20164.261858	30.920628
491.344174	20189.877683	30.925645
492.111912	20215.175464	30.930663
492.826991	20241.290254	30.935680
493.432740	20268.704794	30.940698
493.660292	20297.619158	30.945716
494.148210	20323.200999	30.950733
494.527518	20343.498901	30.955751
495.192810	20376.691752	30.960768
495.475694	20409.306413	30.965786
496.123498	20439.147126	30.970804
496.622621	20466.104776	30.975821
497.194094	20487.996521	30.980839
497.830894	20516.941884	30.985856
498.042360	20549.770149	30.990874
498.629853	20574.110974	30.995892
499.168052	20601.953569	31.000909
499.806027	20616.783824	31.005927
500.367203	20653.936074	31.010944
500.548189	20674.701345	31.015962
501.462685	20699.319662	31.020980
501.900627	20724.025288	31.025997
502.664972	20746.771681	31.031015
502.662588	20780.695308	31.036032
503.144254	20811.548274	31.041050
503.524054	20834.323406	31.046068
503.865684	20865.552219	31.051085
504.855479	20889.950476	31.056103
505.314661	20929.160061	31.061120
505.751223	20955.572163	31.066138
506.410744	20975.542503	31.071156
506.767086	21012.481095	31.076173
507.316108	21030.933420	31.081191
507.916623	21075.333870	31.086208
508.635391	21090.764720	31.091226
509.167744	21115.582421	31.096244
509.402241	21146.923237	31.101261
510.133144	21173.649684	31.106279
510.681320	21197.883709	31.111296
511.255119	21232.128571	31.116314
511.730831	21254.800710	31.121332
511.796790	21276.260713	31.126349
512.149482	21306.812412	31.131367
512.614715	21329.246175	31.136384
513.120887	21374.534033	31.141402
513.847581	21402.209232	31.146420
514.220145	21431.791274	31.151437
514.759898	21459.830718	31.156455
515.479321	21492.852696	31.161472
515.950997	21516.979044	31.166490
516.249876	21544.228599	31.171508
516.771018	21580.586407	31.176525
517.474240	21616.681976	31.181543
517.642815	21629.962632	31.186560
518.328487	21655.117162	31.191578
518.947487	21672.042657	31.196596
519.286224	21718.109448	31.201613
519.920549	21738.021324	31.206631
520.170809	21763.781274	31.211648
520.597173	21803.591695	31.216666
521.198890	21826.826076	31.221684
521.457376	21861.626912	31.226701
522.032749	21891.076779	31.231719
522.446104	21933.138959	31.236736
523.281002	21964.879899	31.241754
523.790528	22005.018912	31.246772
524.024138	22039.672307	31.251789
524.738461	22074.825481	31.256807
525.269470	22105.849671	31.261824
525.904527	22138.045547	31.266842
526.577579	22160.226549	31.271860
527.008271	22209.401566	31.276877
527.723899	22233.187279	31.281895
528.334982	22264.723639	31.286912
528.372389	22298.751060	31.291930
529.271538	22326.703852	31.296948
529.812875	22360.658771	31.301965
530.679225	22388.250294	31.306983
531.111941	22417.976045	31.312000
531.749323	22449.843482	31.317018
532.480623	22471.023646	31.322036
533.120377	22510.795749	31.327053
533.738119	22532.050634	31.332071
534.226061	22552.226378	31.337088
534.461042	22589.306987	31.342106
535.354079	22604.907621	31.347124
535.693775	22632.626203	31.352141
536.098537	22657.876560	31.357159
536.818621	22680.316177	31.362176
537.118658	22711.743993	31.367194
537.855032	22742.951864	31.372212
538.246342	22775.837808	31.377229
538.671938	22803.132441	31.382247
539.342593	22840.480190	31.387264
540.075432	22858.425194	31.392282
540.980681	22886.927579	31.397300
541.271605	22911.532590	31.402317
541.980025	22927.137120	31.407335
542.099877	22956.508261	31.412352
542.858889	22988.319601	31.417370
543.315987	23010.680720	31.422388
543.570992	23038.798597	31.427405
544.135677	23068.555208	31.432423
544.899349	23096.846263	31.437440
544.934042	23132.025611	31.442458
545.652828	23158.200564	31.447476
546.085734	23203.681019	31.452493
546.691937	23235.674668	31.457511
547.452708	23269.148117	31.462528
547.941982	23298.512457	31.467546
548.559656	23331.995786	31.472564
549.014976	23372.935954	31.477581
549.547560	23390.666357	31.482599
550.045168	23425.438804	31.487616
550.765365	23460.827329	31.492634
551.166142	23478.047640	31.497652
551.837627	23512.969946	31.502669
552.324031	23543.598943	31.507687
552.905481	23566.870139	31.512704
552.942239	23600.280602	31.517722
554.333910	23629.706315	31.522740
554.556610	23662.695966	31.527757
554.723722	23688.395606	31.532775
555.286376	23718.210381	31.537792
555.884925	23752.076569	31.542810
556.453287	23782.907954	31.547828
556.964163	23813.034307	31.552845
557.780814	23852.869864	31.557863
558.196321	23879.864227	31.562880
558.292986	23919.856915	31.567898
558.792790	23933.788686	31.572916
559.503768	23972.686809	31.577933
560.179127	24015.559160	31.582951
560.746092	24043.427376	31.587968
561.342402	24091.873338	31.592986
561.996945	24115.335949	31.598004
562.490165	24155.096377	31.603021
563.174852	24194.757382	31.608039
563.664463	24224.818173	31.613056
564.276459	24263.549102	31.618074
564.997685	24291.633644	31.623092
565.684053	24328.381375	31.628109
566.259032	24366.176697	31.633127
566.803883	24388.392911	31.638144
567.327951	24426.897786	31.643162
568.051746	24453.509707	31.648180
568.599333	24478.190206	31.653197
569.182631	24513.292383	31.658215
569.787047	24544.081381	31.663232
570.196818	24573.390535	31.668250
570.832256	24603.201552	31.673268
571.543996	24643.023519	31.678285
571.908635	24676.049488	31.683303
572.613719	24710.981268	31.688320
573.082106	24742.190010	31.693338
574.051419	24777.857837	31.698356
574.809309	24814.102329	31.703373
574.742798	24839.814759	31.708391
575.415617	24868.596535	31.713408
575.985574	24917.996572	31.718426
576.757711	24936.474473	31.723444
577.476775	24976.049488	31.728461
577.922692	25013.872566	31.733479
578.422735	25044.356375	31.738496
578.528565	25082.327640	31.743514
579.535315	25115.165291	31.748532
579.986620	25153.790394	31.753549
580.703394	25190.471749	31.758567
581.574628	25217.548217	31.763584
581.909606	25260.659817	31.768602
582.404495	25275.547582	31.773620
582.695159	25315.158761	31.778637
583.670985	25354.397279	31.783655
584.303716	25390.144191	31.788672
584.879769	25426.121236	31.793690
585.259721	25456.858313	31.798708
586.028558	25501.937469	31.803725
586.554474	25528.714528	31.808743
586.529900	25568.678931	31.813760
587.387444	25602.191694	31.818778
588.260005	25631.177118	31.823796
588.867898	25682.348983	31.828813
589.346554	25715.598960	31.833831
589.849229	25744.952154	31.838848
590.580474	25793.690771	31.843866
591.179928	25832.616292	31.848884
591.723458	25863.404210	31.853901
592.189884	25899.917509	31.858919
592.723988	25928.779411	31.863936
593.625626	25952.584677	31.868954
594.214676	25977.412208	31.873972
595.097698	26008.678059	31.878989
595.296372	26041.397302	31.884007
596.116922	26068.843099	31.889024
596.528544	26101.851411	31.894042
596.601938	26133.794099	31.899060
597.447007	26172.422688	31.904077
598.034876	26213.992546	31.909095
598.487839	26244.466587	31.914112
598.822839	26283.952644	31.919130
599.734907	26317.382219	31.924148
600.098469	26364.460730	31.929165
600.821519	26408.670589	31.934183
601.623227	26426.279375	31.939200
601.959370	26474.632785	31.944218
602.603805	26515.593990	31.949236
603.702867	26555.845739	31.954253
603.856286	26595.954940	31.959271
604.822779	26633.080149	31.964288
604.964398	26671.933627	31.969306
605.792494	26708.157897	31.974324
606.696692	26752.681431	31.979341
606.924394	26789.511816	31.984359
607.618126	26834.555151	31.989376
608.566303	26873.851523	31.994394
609.214985	26916.437187	31.999412
609.913990	26951.165239	32.004429
610.341235	26993.918471	32.009447
611.249325	27022.988819	32.014464
611.951952	27058.203153	32.019482
612.246790	27084.847818	32.024500
613.294742	27123.288443	32.029517
613.820614	27156.735649	32.034535
614.806638	27182.545352	32.039552
615.182455	27217.602573	32.044570
615.256894	27251.973888	32.049588
616.223354	27284.353679	32.054605
616.572199	27326.645861	32.059623
617.539712	27355.005813	32.064640
618.099739	27403.098838	32.069658
618.268741	27443.997329	32.074676
619.052131	27489.603240	32.079693
619.619048	27518.139928	32.084711
620.635096	27548.679437	32.089728
621.011813	27591.391277	32.094746
621.543906	27627.227434	32.099764
622.111131	27663.519550	32.104781
622.796346	27704.280834	32.109799
623.793314	27736.157248	32.114816
624.111730	27773.758957	32.119834
624.930399	27815.504533	32.124852
625.287144	27848.246178	32.129869
625.801851	27899.804834	32.134887
626.867771	27926.032774	32.139904
627.125546	27959.131409	32.144922
627.854564	28004.475204	32.149940
628.666216	28041.001501	32.154957
629.034318	28086.402001	32.159975
629.853680	28119.090592	32.164992
630.868913	28161.014675	32.170010
631.125494	28195.441224	32.175028
631.913317	28224.146568	32.180045
632.787668	28262.395315	32.185063
633.688855	28282.771255	32.190080
634.542883	28312.174275	32.195098
634.854728	28342.597719	32.200116
635.649096	28351.170683	32.205133
636.257867	28375.397597	32.210151
636.649942	28402.888381	32.215168
637.176788	28428.518753	32.220186
637.905163	28451.222684	32.225204
638.603568	28477.293988	32.230221
638.907145	28503.262818	32.235239
639.019678	28526.834416	32.240256
640.232801	28567.211354	32.245274
640.616249	28589.040299	32.250292
641.200051	28627.657596	32.255309
641.531392	28661.118778	32.260327
642.350301	28699.749958	32.265344
642.630044	28733.750289	32.270362
643.574401	28776.969874	32.275380
644.182529	28802.746009	32.280397
644.342333	28847.732040	32.285415
645.529409	28890.547242	32.290432
645.996838	28921.041994	32.295450
646.933778	28964.768811	32.300468
647.692294	29007.423820	32.305485
648.166075	29050.515410	32.310503
648.881619	29087.178731	32.315520
649.558553	29134.625432	32.320538
649.831144	29169.449334	32.325556
650.699594	29212.808148	32.330573
650.924121	29253.101067	32.335591
651.929953	29295.193300	32.340608
652.420826	29340.773308	32.345626
652.796374	29383.596534	32.350644
653.915454	29425.766116	32.355661
654.503162	29469.517097	32.360679
655.142879	29507.204418	32.365696
656.008212	29554.274925	32.370714
656.569723	29606.064431	32.375732
657.354492	29642.806401	32.380749
657.681967	29693.488653	32.385767
658.170702	29731.800540	32.390784
659.239513	29775.761282	32.395802
659.960019	29822.090221	32.400820
661.240322	29858.053319	32.405837
661.711448	29894.307555	32.410855
662.518372	29927.291763	32.415872
663.147705	29964.583312	32.420890
663.871229	30007.479766	32.425908
664.776078	30036.257827	32.430925
664.960579	30082.905182	32.435943
665.913037	30110.575990	32.440960
666.539533	30152.919027	32.445978
666.728929	30193.851419	32.450996
667.785023	30233.763177	32.456013
668.183660	30278.057515	32.461031
668.893238	30315.659520	32.466048
669.298519	30356.103288	32.471066
670.004920	30403.712659	32.476084
670.726386	30434.700868	32.481101
671.373927	30484.076986	32.486119
671.880032	30528.019996	32.491136
672.464515	30566.116154	32.496154
673.179825	30613.509685	32.501172
674.120905	30658.016996	32.506189
674.753026	30702.244071	32.511207
675.635221	30743.423056	32.516224
676.304594	30790.969582	32.521242
677.251790	30828.421524	32.526260
678.077506	30847.749831	32.531277
678.317387	30898.132683	32.536295
678.714066	30931.599967	32.541312
679.586379	30959.783869	32.546330
679.932889	31009.777324	32.551348
680.891359	31041.867210	32.556365
681.220209	31080.453181	32.561383
682.113544	31115.063047	32.566400
682.968103	31156.493726	32.571418
683.400259	31201.556027	32.576436
684.360521	31226.666860	32.581453
684.799763	31268.712785	32.586471
685.408033	31311.623677	32.591488
686.063575	31346.599895	32.596506
686.735727	31391.877892	32.601524
687.565245	31420.834048	32.606541
688.246321	31461.995388	32.611559
688.657464	31514.167241	32.616576
689.769659	31552.953823	32.621594
690.250129	31595.961178	32.626612
691.432159	31640.015634	32.631629
691.730823	31674.055779	32.636647
692.435458	31719.152394	32.641664
693.006052	31755.356385	32.646682
693.588518	31807.268239	32.651700
694.330930	31857.644260	32.656717
695.308934	31898.191002	32.661735
695.935264	31928.203823	32.666752
696.863044	31977.887314	32.671770
697.510245	32027.482105	32.676788
698.244691	32068.737439	32.681805
698.963345	32105.140119	32.686823
699.518119	32157.803166	32.691840
700.482690	32195.684749	32.696858
700.770785	32245.747221	32.701876
701.497151	32281.965666	32.706893
702.314365	32332.444918	32.711911
702.993702	32381.479187	32.716928
703.751114	32421.441942	32.721946
704.411406	32471.914496	32.726964
705.329090	32512.288544	32.731981
705.909416	32558.696135	32.736999
706.781525	32604.476508	32.742016
707.541962	32642.921924	32.747034
708.247335	32698.451929	32.752052
708.917232	32729.963735	32.757069
709.947787	32771.471227	32.762087
710.023395	32820.101626	32.767104
710.829068	32857.933433	32.772122
711.334614	32912.433184	32.777140
712.497067	32946.807974	32.782157
713.375797	32992.701960	32.787175
713.893719	33034.467274	32.792192
714.709817	33075.496860	32.797210
715.735411	33117.770802	32.802228
716.331478	33164.063472	32.807245
716.843240	33211.520091	32.812263
717.444480	33257.552947	32.817280
718.097775	33291.887918	32.822298
718.385082	33348.300686	32.827316
719.407786	33395.538618	32.832333
720.138410	33442.038433	32.837351
720.613512	33490.152619	32.842368
721.711260	33525.619610	32.847386
722.373935	33577.675037	32.852404
722.874423	33618.767757	32.857421
723.971072	33683.691006	32.862439
724.594808	33722.513867	32.867456
725.415383	33777.409098	32.872474
725.919434	33822.541667	32.877492
726.709900	33857.045754	32.882509
727.624846	33906.116245	32.887527
728.081471	33944.478859	32.892544
728.818782	33979.604749	32.897562
729.094542	34016.048501	32.902580
729.912809	34068.953280	32.907597
730.821211	34107.770209	32.912615
731.683412	34149.370024	32.917632
732.396653	34179.486273	32.922650
733.042444	34233.651366	32.927668
733.733306	34271.010547	32.932685
734.672848	34313.414182	32.937703
735.217302	34359.060023	32.942720
736.249540	34394.703130	32.947738
736.629347	34454.442698	32.952756
737.697068	34492.255386	32.957773
738.370828	34543.268238	32.962791
738.979311	34586.103623	32.967808
739.597505	34630.537204	32.972826
740.528931	34669.073367	32.977844
741.038202	34718.430574	32.982861
741.997748	34766.358005	32.987879
742.533448	34812.828148	32.992896
743.197172	34863.577792	32.997914
744.202823	34924.605358	33.002932
744.737954	34967.294935	33.007949
745.449814	35013.997166	33.012967
746.832500	35063.578801	33.017984
748.049649	35092.574188	33.023002
748.932820	35132.705775	33.028020
749.596929	35171.151938	33.033037
750.792738	35209.837373	33.038055
751.388740	35247.693673	33.043072
752.336336	35267.089197	33.048090
752.613889	35299.804411	33.053108
753.574621	35338.830391	33.058125
754.292706	35369.074040	33.063143
755.079189	35409.423626	33.068160
756.227811	35438.114076	33.073178
756.396873	35483.454404	33.078196
757.115523	35519.667000	33.083213
757.650557	35560.479884	33.088231
758.404969	35608.169464	33.093248
759.158713	35645.192437	33.098266
759.839908	35693.285696	33.103284
760.408576	35743.192411	33.108301
761.072065	35784.674816	33.113319
761.583613	35836.026013	33.118336
762.683101	35889.719628	33.123354
763.527395	35930.111736	33.128372
763.954067	35976.658412	33.133389
765.203941	36031.138186	33.138407
765.459224	36076.478922	33.143424
766.411699	36119.067526	33.148442
767.728971	36172.607614	33.153460
768.218264	36212.746019	33.158477
769.042830	36261.330285	33.163495
769.755792	36316.305871	33.168512
770.733764	36354.268733	33.173530
771.599990	36396.978894	33.178548
772.180032	36441.795314	33.183565
773.180374	36489.302926	33.188583
773.646055	36533.372340	33.193600
774.456281	36573.151331	33.198618
774.948895	36617.191407	33.203636
775.822760	36665.465360	33.208653
776.875136	36717.682480	33.213671
777.301466	36759.399944	33.218688
778.123531	36798.481940	33.223706
778.819893	36837.400317	33.228724
779.244448	36889.969104	33.233741
780.465533	36919.655623	33.238759
781.450521	36966.003211	33.243776
782.628456	36990.435567	33.248794
783.522327	37019.787743	33.253812
784.435461	37047.941826	33.258829
785.555297	37078.365286	33.263847
785.326915	37122.924005	33.268864
786.508053	37147.861913	33.273882
787.440078	37186.092713	33.278900
787.706746	37211.515359	33.283917
788.753454	37246.244108	33.288935
789.366506	37288.420270	33.293952
789.988806	37333.984435	33.298970
790.906493	37362.745272	33.303988
791.578701	37411.457193	33.309005
792.514068	37453.564237	33.314023
792.530311	37502.183055	33.319040
793.542432	37541.363120	33.324058
794.383975	37592.679516	33.329076
794.716483	37649.242079	33.334093
796.152032	37699.991449	33.339111
796.801507	37754.740383	33.344128
797.402859	37805.570044	33.349146
798.372031	37857.771361	33.354164
799.099060	37904.787415	33.359181
800.110174	37960.852470	33.364199
800.875681	38010.291005	33.369216
801.717448	38056.505292	33.374234
802.434561	38107.077239	33.379252
803.147640	38165.080276	33.384269
804.476873	38210.010735	33.389287
804.586812	38264.295290	33.394304
805.506679	38318.225500	33.399322
806.362110	38371.476646	33.404340
807.194236	38433.376168	33.409357
808.401929	38483.340982	33.414375
808.643593	38539.098016	33.419392
809.683290	38592.371444	33.424410
810.798585	38650.407661	33.429428
811.298032	38697.492704	33.434445
812.421974	38748.337616	33.439463
812.614709	38811.438697	33.444480
813.643029	38872.707988	33.449498
814.435529	38920.183976	33.454516
815.218948	38990.547798	33.459533
816.116916	39046.121157	33.464551
816.935209	39098.235278	33.469568
818.253288	39145.502981	33.474586
819.052827	39200.605204	33.479604
819.663277	39259.771897	33.484621
820.553574	39296.406690	33.489639
821.237078	39355.562205	33.494656
822.442782	39410.329427	33.499674
823.152072	39469.626669	33.504692
823.831915	39516.818052	33.509709
825.086510	39571.015182	33.514727
825.808143	39617.232652	33.519744
826.698441	39658.857788	33.524762
827.731174	39704.375345	33.529780
828.162966	39752.997396	33.534797
829.189541	39799.692410	33.539815
829.658517	39852.470165	33.544832
830.675230	39905.604974	33.549850
831.563263	39947.085562	33.554868
832.049703	40008.284815	33.559885
833.351589	40053.394152	33.564903
834.136966	40096.402595	33.569920
834.959512	40136.091386	33.574938
835.720710	40171.906748	33.579956
836.429631	40225.394101	33.584973
837.684852	40265.420132	33.589991
838.300480	40296.116834	33.595008
839.127048	40333.591846	33.600026
839.558042	40373.563734	33.605044
840.527848	40429.654312	33.610061
841.214010	40472.913036	33.615079
842.192131	40521.400662	33.620096
842.474365	40575.708291	33.625114
843.640419	40622.939782	33.630132
844.430647	40675.213871	33.635149
845.272927	40717.790896	33.640167
846.309758	40766.472256	33.645184
847.089480	40826.906897	33.650202
847.628472	40874.483778	33.655220
848.778103	40934.025961	33.660237
850.003919	40983.677485	33.665255
850.299833	41036.826732	33.670272
851.060423	41090.074109	33.675290
852.067917	41150.290566	33.680308
852.831518	41206.111851	33.685325
854.232997	41252.074549	33.690343
855.029841	41310.085527	33.695360
855.409659	41360.654631	33.700378
856.324917	41415.719047	33.705396
857.070885	41472.081365	33.710413
858.355561	41525.133893	33.715431
859.358014	41588.217421	33.720448
860.481299	41640.517563	33.725466
861.352768	41693.521357	33.730484
861.965721	41752.466736	33.735501
863.027435	41794.480221	33.740519
863.907892	41851.847066	33.745536
864.579372	41899.753291	33.750554
865.813009	41953.706643	33.755572
866.660812	42004.741559	33.760589
867.483713	42049.797212	33.765607
868.505303	42106.889632	33.770624
869.122254	42158.745334	33.775642
869.826199	42203.984376	33.780660
870.673347	42255.076900	33.785677
871.900122	42309.531867	33.790695
872.562573	42368.686194	33.795712
873.499697	42421.814288	33.800730
874.243242	42465.137539	33.805748
874.697825	42528.050232	33.810765
875.632778	42582.108822	33.815783
876.878423	42638.370591	33.820800
877.675918	42695.702028	33.825818
878.587972	42746.235253	33.830836
879.455916	42802.164431	33.835853
880.400932	42855.456787	33.840871
881.387413	42908.230448	33.845888
882.078243	42963.485686	33.850906
883.239491	43016.953301	33.855924
883.982010	43086.868659	33.860941
884.909748	43121.543225	33.865959
885.679630	43176.660115	33.870976
886.548419	43248.991394	33.875994
887.401552	43292.128330	33.881012
887.912383	43351.625290	33.886029
889.415876	43403.522205	33.891047
890.465330	43463.067955	33.896064
891.236695	43512.688831	33.901082
892.253865	43553.555132	33.906100
893.025795	43609.786024	33.911117
893.916777	43638.660564	33.916135
894.918452	43685.652403	33.921152
895.251468	43726.980367	33.926170
896.304838	43769.315193	33.931188
897.218666	43819.483727	33.936205
898.082116	43860.109001	33.941223
899.108085	43915.212932	33.946240
900.219235	43961.783392	33.951258
900.978142	44006.783483	33.956276
901.619536	44062.333844	33.961293
902.136153	44109.908565	33.966311
902.898814	44152.137833	33.971328
903.846227	44218.469790	33.976346
904.875723	44271.733351	33.981364
905.795449	44335.084378	33.986381
906.759722	44384.038123	33.991399
907.815460	44440.220354	33.996416
908.753796	44502.436678	34.001434
909.343440	44558.951536	34.006452
910.213175	44621.887395	34.011469
910.979041	44690.823686	34.016487
912.228430	44749.506604	34.021504
912.984171	44815.958911	34.026522
913.663484	44876.882134	34.031540
914.572254	44935.188732	34.036557
916.294141	44997.574729	34.041575
917.072650	45055.440265	34.046592
917.961979	45120.468261	34.051610
918.967088	45176.729857	34.056628
919.839894	45242.197268	34.061645
920.862062	45292.263597	34.066663
922.025285	45342.257345	34.071680
922.562112	45408.764668	34.076698
923.590057	45466.623840	34.081716
924.783861	45518.593168	34.086733
925.532246	45574.105236	34.091751
926.870399	45635.319565	34.096768
927.664274	45690.445248	34.101786
928.718532	45744.669978	34.106804
929.602380	45801.451876	34.111821
930.317147	45858.987871	34.116839
931.208010	45912.915970	34.121856
932.374631	45971.267131	34.126874
933.392905	46017.236486	34.131892
934.099223	46073.237147	34.136909
935.124344	46141.163111	34.141927
936.211560	46192.233424	34.146944
936.722748	46260.733647	34.151962
937.765420	46309.470575	34.156980
939.068412	46378.928929	34.161997
940.162217	46439.620694	34.167015
940.959712	46481.608517	34.172032
941.736210	46542.843677	34.177050
942.721775	46594.658321	34.182068
943.844951	46652.031179	34.187085
944.567472	46713.914194	34.192103
945.826250	46767.571647	34.197120
946.407867	46824.922195	34.202138
947.739951	46875.816544	34.207156
948.698932	46930.198227	34.212173
949.722733	46985.468216	34.217191
950.472265	47026.433391	34.222208
951.233807	47089.753706	34.227226
951.991810	47142.984362	34.232244
952.958504	47197.011210	34.237261
954.111105	47263.490857	34.242279
955.208001	47309.159531	34.247296
955.728086	47359.112962	34.252314
956.758609	47406.595227	34.257332
957.788638	47455.077232	34.262349
958.305296	47510.611375	34.267367
959.477317	47552.485612	34.272384
960.499418	47599.678588	34.277402
961.186916	47657.887711	34.282420
962.346769	47711.683099	34.287437
963.231765	47760.903353	34.292455
964.285730	47805.377729	34.297472
965.195976	47862.508636	34.302490
966.401024	47916.556820	34.307508
967.564235	47961.552147	34.312525
968.512903	48015.722954	34.317543
969.836859	48071.587576	34.322560
970.348611	48118.108683	34.327578
971.390557	48168.665453	34.332596
972.278217	48226.382855	34.337613
973.446861	48285.486216	34.342631
974.310773	48324.164587	34.347648
974.812649	48389.604308	34.352666
976.192610	48446.903552	34.357684
976.943082	48508.097485	34.362701
977.856806	48570.847686	34.367719
979.176632	48627.802508	34.372736
979.838141	48677.584854	34.377754
980.709983	48734.382323	34.382772
981.947133	48796.133500	34.387789
983.208436	48862.411007	34.392807
984.127803	48916.082405	34.397824
985.261666	48984.778061	34.402842
986.284532	49038.446195	34.407860
987.417762	49098.556843	34.412877
988.063104	49161.407630	34.417895
988.912579	49212.775052	34.422912
989.871614	49278.632907	34.427930
990.916659	49336.518281	34.432948
992.063816	49404.472873	34.437965
992.890953	49461.045053	34.442983
994.057209	49520.455678	34.448000
994.797953	49587.936658	34.453018
995.829380	49656.365657	34.458036
996.992163	49720.180908	34.463053
997.936245	49776.090203	34.468071
998.992795	49835.531476	34.473088
1000.005352	49903.097365	34.478106
1001.236264	49969.844710	34.483124
1002.862250	50016.884872	34.488141
1003.143097	50071.044900	34.493159
1004.029638	50134.733724	34.498176
1005.201193	50206.875406	34.503194
1006.223446	50263.703734	34.508212
1007.826832	50316.518388	34.513229
1008.416919	50380.507393	34.518247
1009.481243	50428.813189	34.523264
1010.246706	50486.061902	34.528282
1011.371030	50541.938513	34.533300
1012.796298	50598.483116	34.538317
1013.660627	50671.041333	34.543335
1014.655271	50712.316421	34.548352
1015.615931	50786.783403	34.553370
1016.594249	50840.114725	34.558388
1017.812051	50889.061823	34.563405
1018.537662	50946.627955	34.568423
1019.426673	51005.952954	34.573440
1020.193012	51063.677511	34.578458
1021.423571	51130.105580	34.583476
1022.513213	51169.152036	34.588493
1023.399198	51230.698993	34.593511
1024.544817	51276.355317	34.598528
1025.394181	51342.875317	34.603546
1026.212875	51384.843535	34.608564
1027.042648	51434.295461	34.613581
1028.071330	51506.849549	34.618599
1029.172595	51558.802875	34.623616
1030.058295	51621.844201	34.628634
1030.591514	51679.878875	34.633652
1031.989319	51741.385019	34.638669
1032.820442	51807.086627	34.643687
1034.246911	51870.138874	34.648704
1035.052169	51933.902329	34.653722
1036.276431	51995.936198	34.658740
1037.358385	52058.688551	34.663757
1038.294573	52128.209151	34.668775
1039.589500	52189.840161	34.673792
1040.920051	52248.536047	34.678810
1041.805461	52313.983808	34.683828
1043.257543	52362.884686	34.688845
1043.986764	52434.045839	34.693863
1044.795511	52484.041147	34.698880
1046.144313	52550.979972	34.703898
1047.208537	52608.497208	34.708916
1048.302303	52670.945630	34.713933
1049.324832	52735.847901	34.718951
1050.173321	52802.195032	34.723968
1051.439626	52865.388954	34.728986
1052.530446	52928.192883	34.734004
1053.604576	52986.589071	34.739021
1054.812245	53057.993609	34.744039
1055.889773	53113.054786	34.749056
1056.687681	53179.676679	34.754074
1057.660352	53248.163452	34.759092
1058.915779	53312.163932	34.764109
1059.733665	53379.662851	34.769127
1061.104451	53448.378966	34.774144
1062.437435	53513.247443	34.779162
1063.177786	53580.341430	34.784180
1064.638842	53628.800596	34.789197
1065.056827	53696.698423	34.794215
1066.736955	53758.108734	34.799232
1067.715940	53827.817529	34.804250
1068.574441	53880.320283	34.809268
1069.667972	53942.196273	34.814285
1070.740324	54019.377188	34.819303
1072.073418	54085.879893	34.824320
1073.526104	54141.334048	34.829338
1074.491899	54199.686937	34.834356
1075.853236	54258.731100	34.839373
1076.702669	54319.133857	34.844391
1077.555247	54377.979530	34.849408
1078.915157	54429.607650	34.854426
1079.935420	54486.484567	34.859444
1081.064606	54541.623274	34.864461
1082.330498	54608.631583	34.869479
1083.218506	54660.251823	34.874496
1084.720722	54706.605770	34.879514
1085.460441	54763.109606	34.884532
1086.636578	54815.064775	34.889549
1087.397962	54878.090031	34.894567
1088.369343	54940.449738	34.899584
1089.755420	54999.188121	34.904602
1090.938810	55053.015886	34.909620
1092.288667	55100.451307	34.914637
1093.389250	55160.095454	34.919655
1094.435599	55207.490010	34.924672
1095.404911	55258.592550	34.929690
1096.049869	55315.656791	34.934708
1096.831606	55358.245453	34.939725
1097.858075	55414.073100	34.944743
1098.822591	55462.771996	34.949760
1099.760401	55515.911481	34.954778
1100.695238	55583.170566	34.959796
1101.953571	55642.784901	34.964813
1102.923139	55705.912664	34.969831
1103.560569	55768.630606	34.974848
1104.708881	55829.192940	34.979866
1105.955461	55896.467391	34.984884
1107.327580	55962.323744	34.989901
1107.889118	56032.053761	34.994919
1109.521140	56100.192432	34.999936
1110.863992	56167.053868	35.004954
1111.531109	56225.882534	35.009972
1113.048331	56293.368885	35.014989
1113.954161	56362.913064	35.020007
1115.092196	56436.420885	35.025024
1116.654461	56502.824884	35.030042
1117.609429	56572.956889	35.035060
1118.750252	56636.636229	35.040077
1119.743761	56704.047513	35.045095
1120.880631	56770.499869	35.050112
1122.527775	56825.372927	35.055130
1123.425220	56902.755156	35.060148
1124.665376	56963.356624	35.065165
1125.792678	57021.931664	35.070183
1126.896752	57085.725546	35.075200
1128.477639	57151.603130	35.080218
1129.735958	57214.189688	35.085236
1130.872832	57282.902917	35.090253
1132.204527	57331.554475	35.095271
1133.105238	57398.627817	35.100288
1134.530290	57447.961191	35.105306
1135.556348	57505.876057	35.110324
1136.469976	57566.485867	35.115341
1137.698105	57637.128852	35.120359
1138.960232	57694.798356	35.125376
1140.237307	57753.959333	35.130394
1141.540782	57820.932823	35.135412
1142.606342	57874.266417	35.140429
1143.619094	57936.532541	35.145447
1144.709963	57992.989052	35.150464
1146.233960	58049.169022	35.155482
1147.217018	58108.117403	35.160500
1148.554599	58165.421786	35.165517
1149.552190	58222.830167	35.170535
1150.683825	58285.926703	35.175552
1152.092471	58330.941567	35.180570
1152.916940	58389.092656	35.185588
1153.921014	58455.070448	35.190605
1154.818279	58516.349788	35.195623
1156.053118	58581.544937	35.200640
1157.327950	58633.385369	35.205658
1158.366001	58701.940896	35.210676
1159.752025	58770.391506	35.215693
1160.354139	58830.205121	35.220711
1161.355510	58899.089749	35.225728
1163.116468	58954.816991	35.230746
1164.243969	59027.201411	35.235764
1165.447047	59087.700103	35.240781
1166.541581	59151.260428	35.245799
1167.834720	59219.492658	35.250816
1169.453936	59269.558911	35.255834
1170.231815	59333.789581	35.260852
1171.492570	59386.463001	35.265869
1173.124784	59442.401409	35.270887
1173.541869	59488.959840	35.275904
1174.554415	59529.614569	35.280922
1175.783154	59588.781279	35.285940
1176.824026	59633.843488	35.290957
1177.873261	59678.955109	35.295975
1178.765636	59741.643490	35.300992
1180.430800	59794.988725	35.306010
1181.388550	59857.192444	35.311028
1182.619343	59909.327336	35.316045
1183.818182	59970.797336	35.321063
1184.713211	60020.927876	35.326080
1186.076425	60078.207455	35.331098
1186.963743	60141.201483	35.336116
1188.170253	60204.576128	35.341133
1189.268984	60272.898716	35.346151
1190.466668	60340.199564	35.351168
1191.821840	60403.329909	35.356186
1192.982704	60477.675665	35.361204
1194.153175	60536.258792	35.366221
1195.381356	60613.126365	35.371239
1196.477210	60675.677681	35.376256
1197.725322	60746.674742	35.381274
1198.764926	60826.750122	35.386292
1200.238864	60895.775303	35.391309
1201.514858	60977.687834	35.396327
1202.293111	61045.733591	35.401344
1204.077922	61103.076172	35.406362
1205.330757	61184.068837	35.411380
1206.436875	61246.841555	35.416397
1207.906197	61320.489583	35.421415
1209.308927	61394.072297	35.426432
1210.297480	61452.996268	35.431450
1211.538789	61519.723817	35.436468
1212.864585	61586.014202	35.441485
1214.126952	61657.087625	35.446503
1215.589014	61734.194289	35.451520
1216.798477	61783.855090	35.456538
1217.901626	61850.978646	35.461556
1219.398316	61921.224874	35.466573
1220.628043	61986.296985	35.471591
1221.996913	62052.980688	35.476608
1223.644599	62111.929655	35.481626
1224.565449	62176.139062	35.486644
1225.504893	62228.533398	35.491661
1226.332432	62284.623271	35.496679
1227.586391	62349.901446	35.501696
1228.966721	62414.400370	35.506714
1230.210336	62487.935293	35.511732
1231.355291	62559.738696	35.516749
1232.945933	62623.730464	35.521767
1234.115984	62698.689207	35.526784
1235.633670	62756.001494	35.531802
1236.943210	62815.581144	35.536820
1238.241376	62885.456043	35.541837
1239.933041	62943.146678	35.546855
1240.495207	63005.546895	35.551872
1241.846109	63056.422558	35.556890
1243.174541	63120.437666	35.561908
1244.086576	63180.105741	35.566925
1245.983062	63245.336336	35.571943
1246.392925	63303.222137	35.576960
1247.922986	63358.337174	35.581978
1248.809232	63430.930603	35.586996
1250.000219	63500.330223	35.592013
1251.174272	63569.644057	35.597031
1252.675582	63644.927303	35.602048
1253.941774	63704.572847	35.607066
1254.865431	63768.621335	35.612084
1256.063768	63828.556347	35.617101
1257.378376	63884.725521	35.622119
1258.538072	63952.744871	35.627136
1259.918787	63991.975572	35.632154
1260.876787	64061.356248	35.637172
1261.786812	64126.933500	35.642189
1263.515053	64188.426095	35.647207
1264.276706	64254.058560	35.652224
1265.674060	64322.877380	35.657242
1266.872296	64388.739403	35.662260
1267.863520	64454.095883	35.667277
1269.482273	64525.248341	35.672295
1270.461488	64601.318925	35.677312
1272.018500	64666.986236	35.682330
1273.607257	64750.463982	35.687348
1274.987795	64806.175408	35.692365
1276.486249	64870.339324	35.697383
1277.349907	64949.239997	35.702400
1278.487208	65012.834044	35.707418
1280.296989	65083.135152	35.712436
1281.374817	65148.733122	35.717453
1282.976124	65219.307825	35.722471
1284.274358	65289.240082	35.727488
1285.825037	65350.592387	35.732506
1287.035913	65412.498190	35.737524
1288.290808	65488.737228	35.742541
1289.574421	65547.985571	35.747559
1291.105822	65614.431766	35.752576
1292.452651	65674.158009	35.757594
1293.660738	65748.176588	35.762612
1294.394135	65815.083783	35.767629
1296.288961	65867.842691	35.772647
1297.545030	65941.423803	35.777664
1299.115863	66009.992159	35.782682
1300.502285	66073.220658	35.787700
1301.538441	66129.489092	35.792717
1303.307558	66208.429235	35.797735
1304.204499	66280.794960	35.802752
1305.448744	66340.279252	35.807770
1306.912136	66406.649536	35.812788
1308.030535	66474.846781	35.817805
1309.471980	66530.096625	35.822823
1310.784247	66605.006787	35.827840
1312.481921	66671.727307	35.832858
1313.847292	66745.850808	35.837876
1314.844023	66808.850897	35.842893
1316.543891	66870.823014	35.847911
1317.181641	66932.632307	35.852928
1318.614504	66995.716544	35.857946
1319.968975	67068.500415	35.862964
1321.431004	67136.955888	35.867981
1322.722427	67213.283034	35.872999
1323.881643	67278.747148	35.878016
1325.306500	67353.641888	35.883034
1326.913893	67417.073412	35.888052
1327.810528	67496.293425	35.893069
1329.251502	67563.531337	35.898087
1330.570608	67638.367487	35.903104
1332.063648	67703.894404	35.908122
1333.203388	67767.127741	35.913140
1334.632799	67833.481738	35.918157
1336.039349	67903.423236	35.923175
1337.360002	67982.141490	35.928192
1338.443307	68045.169068	35.933210
1339.854047	68114.527965	35.938228
1341.252733	68183.065806	35.943245
1342.627213	68250.562871	35.948263
1344.168444	68317.977026	35.953280
1345.343598	68369.891351	35.958298
1346.759877	68423.540953	35.963316
1347.752406	68491.415033	35.968333
1348.891033	68537.269494	35.973351
1350.213524	68597.430641	35.978368
1351.850581	68655.288531	35.983386
1353.010746	68719.204862	35.988404
1354.173263	68780.581879	35.993421
1355.664657	68839.868675	35.998439
1356.367936	68911.562979	36.003456
1357.763949	68980.521274	36.008474
1359.334003	69055.493235	36.013492
1360.696850	69125.432237	36.018509
1362.145937	69193.281022	36.023527
1363.527467	69276.229835	36.028544
1364.642253	69344.137678	36.033562
1366.333593	69413.278855	36.038580
1367.679937	69495.239741	36.043597
1368.915656	69559.253971	36.048615
1370.165027	69644.599197	36.053632
1371.380080	69721.578959	36.058650
1373.199936	69797.121856	36.063668
1374.706567	69870.111471	36.068685
1376.131196	69940.188645	36.073703
1377.491623	70016.063717	36.078720
1378.700238	70098.700288	36.083738
1380.417614	70171.087859	36.088756
1382.006599	70255.033158	36.093773
1383.226802	70324.877412	36.098791
1384.742910	70408.328029	36.103808
1386.146437	70479.448461	36.108826
1387.564420	70553.087105	36.113844
1388.847965	70623.682129	36.118861
1390.510524	70701.322967	36.123879
1392.204619	70778.313193	36.128896
1393.484922	70849.859199	36.133914
1395.447095	70916.144054	36.138932
1396.194309	70995.360179	36.143949
1398.078752	71058.807953	36.148967
1399.499534	71121.859853	36.153984
1400.483066	71191.920784	36.159002
1402.178925	71265.555938	36.164020
1403.481096	71334.376857	36.169037
1404.950263	71398.853008	36.174055
1406.260989	71471.257181	36.179072
1407.776227	71548.201681	36.184090
1409.494462	71611.638819	36.189108
1410.633230	71681.170149	36.194125
1412.342753	71755.197164	36.199143
1413.744427	71824.396420	36.204160
1414.970159	71887.024741	36.209178
1417.012194	71947.650959	36.214196
1418.328480	72006.516433	36.219213
1419.904741	72066.607892	36.224231
1420.950333	72139.283387	36.229248
1422.243308	72200.065432	36.234266
1423.627056	72258.350963	36.239284
1425.089358	72329.112585	36.244301
1426.617116	72401.536013	36.249319
1427.774504	72474.055609	36.254336
1429.074291	72532.924843	36.259354
1430.409162	72603.415837	36.264372
1432.076031	72672.284501	36.269389
1433.387838	72743.754742	36.274407
1434.730429	72813.497807	36.279424
1436.168500	72887.697154	36.284442
1437.593277	72959.669596	36.289460
1438.710466	73027.067320	36.294477
1440.474734	73097.543083	36.299495
1441.421712	73154.619698	36.304512
1442.747041	73216.386965	36.309530
1444.122205	73271.471577	36.314548
1445.352613	73339.764329	36.319565
1446.607526	73406.406828	36.324583
1448.028281	73484.853699	36.329600
1449.282393	73558.729067	36.334618
1451.194704	73636.757460	36.339636
1452.553591	73703.422429	36.344653
1454.201950	73765.786390	36.349671
1455.668486	73838.438658	36.354688
1456.762041	73924.474488	36.359706
1458.249219	74004.521119	36.364724
1459.882930	74076.045893	36.369741
1461.277568	74147.519614	36.374759
1463.089470	74231.176702	36.379776
1464.703876	74294.902531	36.384794
1466.275699	74372.796379	36.389812
1467.621332	74443.797234	36.394829
1469.409231	74518.757039	36.399847
1470.891885	74588.672837	36.404864
1472.564008	74664.512504	36.409882
1474.290012	74726.461227	36.414900
1475.407588	74796.523378	36.419917
1477.308612	74864.056397	36.424935
1478.630926	74940.952276	36.429952
1480.021190	75008.958276	36.434970
1481.856306	75077.097490	36.439988
1483.273614	75151.762400	36.445005
1484.556753	75221.419739	36.450023
1486.764234	75287.955839	36.455040
1487.832780	75355.911737	36.460058
1489.464274	75423.754361	36.465076
1490.682054	75500.224856	36.470093
1492.074131	75569.080685	36.475111
1493.828497	75646.974996	36.480128
1495.041714	75721.863440	36.485146
1496.834839	75791.607105	36.490164
1498.019739	75871.934634	36.495181
1499.481923	75943.617912	36.500199
1501.261960	76023.257379	36.505216
1502.507826	76095.798294	36.510234
1503.958095	76168.560760	36.515252
1505.455944	76249.081107	36.520269
1507.036768	76324.699065	36.525287
1508.746006	76397.535620	36.530304
1510.013555	76477.611328	36.535322
1511.564826	76548.256194	36.540340
1513.457877	76619.088434	36.545357
1514.866014	76695.329833	36.550375
1516.391892	76771.629023	36.555392
1517.625486	76853.408623	36.560410
1519.542892	76927.316111	36.565428
1520.800898	77003.797224	36.570445
1522.538125	77078.164028	36.575463
1524.130814	77149.272685	36.580480
1525.413920	77235.036055	36.585498
1526.825803	77307.832918	36.590516
1528.303454	77391.210096	36.595533
1529.585525	77465.319829	36.600551
1531.209415	77537.007342	36.605568
1532.632218	77625.080990	36.610586
1534.541265	77694.469369	36.615604
1535.937406	77777.784476	36.620621
1537.529336	77846.323437	36.625639
1539.357777	77928.025823	36.630656
1540.844395	78007.438328	36.635674
1542.526715	78060.635105	36.640692
1543.609816	78116.028710	36.645709
1545.051616	78184.807378	36.650727
1546.770228	78239.557028	36.655744
1547.478117	78311.630638	36.660762
1549.568593	78375.443598	36.665780
1550.724242	78447.308130	36.670797
1552.129739	78518.601670	36.675815
1553.869604	78589.108287	36.680832
1554.913649	78670.200881	36.685850
1556.591361	78738.449938	36.690868
1558.230686	78820.627984	36.695885
1559.651784	78911.645147	36.700903
1561.306253	78984.687208	36.705920
1562.629187	79073.971991	36.710938
1564.293409	79166.320166	36.715956
1566.164129	79249.666807	36.720973
1567.367728	79329.621509	36.725991
1569.334925	79415.170599	36.731008
1570.747457	79506.254406	36.736026
1572.478344	79590.308083	36.741044
1574.670283	79674.391206	36.746061
1576.067000	79757.129438	36.751079
1577.573841	79834.555003	36.756096
1579.310920	79916.252250	36.761114
1580.932088	80000.666409	36.766132
1582.632349	80082.407915	36.771149
1584.149685	80177.278281	36.776167
1585.974029	80252.970312	36.781184
1587.469492	80343.397752	36.786202
1589.110410	80418.599500	36.791220
1590.692746	80503.743417	36.796237
1592.191425	80591.257200	36.801255
1594.070765	80663.064895	36.806272
1595.395060	80763.858769	36.811290
1597.197430	80841.063508	36.816308
1598.786229	80918.149853	36.821325
1600.395413	81012.210499	36.826343
1602.057109	81096.900367	36.831360
1603.553126	81177.422754	36.836378
1605.594113	81257.403970	36.841396
1607.325317	81341.868316	36.846413
1608.591247	81420.438259	36.851431
1610.746663	81495.232968	36.856448
1611.605792	81583.204702	36.861466
1613.476484	81665.785721	36.866484
1615.165184	81755.706026	36.871501
1616.659862	81839.106601	36.876519
1618.679081	81911.199687	36.881536
1620.049032	81999.852977	36.886554
1621.594697	82077.848834	36.891572
1623.401386	82173.174808	36.896589
1625.117249	82255.465036	36.901607
1626.721902	82337.050708	36.906624
1628.377452	82417.247592	36.911642
1629.978343	82500.810884	36.916660
1631.774615	82583.951065	36.921677
1633.208004	82656.631889	36.926695
1635.170183	82743.623702	36.931712
1636.460502	82829.783321	36.936730
1638.139133	82908.356171	36.941748
1639.609039	82984.782580	36.946765
1641.237944	83069.800274	36.951783
1643.060007	83157.575520	36.956800
1644.405548	83242.828140	36.961818
1646.133594	83321.369059	36.966836
1647.739957	83399.016950	36.971853
1649.151664	83486.426630	36.976871
1650.843334	83549.477583	36.981888
1652.267394	83626.875871	36.986906
1653.922161	83695.710802	36.991924
1655.445387	83771.725516	36.996941
1657.033620	83849.592877	37.001959
1658.867461	83924.013537	37.006976
1660.285729	84000.184665	37.011994
1661.931863	84077.372027	37.017012
1663.405354	84152.153780	37.022029
1664.500160	84249.676183	37.027047
1666.544637	84329.108016	37.032064
1668.128239	84419.864162	37.037082
1669.902044	84512.871641	37.042100
1671.727537	84589.576151	37.047117
1673.337201	84681.292059	37.052135
1674.933736	84779.472672	37.057152
1676.674147	84870.877283	37.062170
1678.281385	84955.029658	37.067188
1680.203806	85044.011446	37.072205
1681.894596	85142.533346	37.077223
1683.793520	85224.283970	37.082240
1685.277709	85320.228485	37.087258
1687.043891	85412.416416	37.092276
1689.119960	85501.096794	37.097293
1690.674785	85595.472561	37.102311
1692.723474	85677.796600	37.107328
1694.421115	85775.762035	37.112346
1695.819130	85865.373310	37.117364
1697.904004	85950.847734	37.122381
1699.473908	86047.098040	37.127399
1700.850211	86125.904433	37.132416
1702.951359	86220.310784	37.137434
1705.038331	86313.376432	37.142452
1706.827786	86405.057003	37.147469
1708.471416	86485.875402	37.152487
1710.518387	86576.743219	37.157504
1712.137131	86656.539549	37.162522
1713.860645	86739.728508	37.167540
1715.845414	86828.401893	37.172557
1717.537679	86912.952161	37.177575
1719.301130	87002.129582	37.182592
1720.425417	87086.579157	37.187610
1722.107967	87178.570355	37.192628
1724.382192	87260.014537	37.197645
1725.696219	87350.365850	37.202663
1727.388208	87444.257269	37.207680
1729.171297	87535.283420	37.212698
1730.700796	87632.242267	37.217716
1732.835024	87717.587429	37.222733
1734.408926	87815.883226	37.227751
1736.258733	87899.461244	37.232768
1738.039777	87983.100951	37.237786
1739.826934	88067.044085	37.242804
1741.949198	88162.720682	37.247821
1743.544958	88248.050271	37.252839
1745.433947	88333.613021	37.257856
1747.526440	88418.687948	37.262874
1748.997942	88493.988110	37.267892
1751.119051	88572.773245	37.272909
1752.746575	88649.899637	37.277927
1754.389863	88739.063118	37.282944
1756.129307	88819.150594	37.287962
1757.748606	88900.739839	37.292980
1759.613641	88976.714684	37.297997
1761.039248	89052.593741	37.303015
1762.804085	89135.035302	37.308032
1764.414428	89212.229215	37.313050
1766.039793	89296.910865	37.318068
1767.951021	89363.856125	37.323085
1768.803278	89450.598209	37.328103
1771.021870	89531.423719	37.333120
1772.500999	89596.561469	37.338138
1773.906111	89672.660765	37.343156
1776.182857	89748.953361	37.348173
1777.801065	89836.070967	37.353191
1778.916768	89915.942176	37.358208
1780.895120	90003.232033	37.363226
1782.548962	90088.139601	37.368244
1784.291165	90179.585844	37.373261
1785.996368	90278.236795	37.378279
1787.824281	90378.541797	37.383296
1789.593255	90463.102897	37.388314
1791.439805	90563.709772	37.393332
1793.820398	90655.615214	37.398349
1795.438545	90758.235601	37.403367
1797.115140	90845.739899	37.408384
1799.147413	90932.909965	37.413402
1800.912864	91050.159371	37.418420
1802.980786	91126.906407	37.423437
1804.660768	91237.516058	37.428455
1806.159228	91325.290434	37.433472
1808.175421	91426.697467	37.438490
1809.951127	91533.947251	37.443508
1811.958158	91619.260149	37.448525
1813.922138	91730.777731	37.453543
1815.665016	91825.308721	37.458560
1817.773458	91929.554725	37.463578
1819.297393	92026.085128	37.468596
1821.471288	92123.261919	37.473613
1823.361330	92226.313701	37.478631
1824.946011	92313.557796	37.483648
1826.864921	92409.393884	37.488666
1828.802095	92523.504185	37.493684
1830.925513	92617.914721	37.498701
1832.653737	92712.729609	37.503719
1834.146072	92818.786158	37.508736
1836.198282	92924.197773	37.513754
1837.916234	93022.830337	37.518772
1840.268080	93122.885006	37.523789
1842.192791	93225.098200	37.528807
1843.802310	93323.774052	37.533824
1845.488140	93426.405548	37.538842
1847.183120	93533.193360	37.543860
1849.404365	93621.672458	37.548877
1851.312557	93719.149415	37.553895
1853.239277	93821.871289	37.558912
1855.006940	93922.298838	37.563930
1856.962639	94024.497171	37.568948
1858.637624	94122.734388	37.573965
1860.446033	94226.300017	37.578983
1862.544708	94323.001237	37.584000
1864.464215	94423.546087	37.589018
1866.557502	94521.186750	37.594036
1867.997622	94617.459577	37.599053
1869.811346	94727.820104	37.604071
1871.555703	94824.692419	37.609088
1873.531254	94941.429535	37.614106
1875.245776	95033.338338	37.619124
1877.337724	95133.021917	37.624141
1879.000147	95243.357251	37.629159
1880.616708	95356.590227	37.634176
1882.720060	95454.282957	37.639194
1884.349180	95567.045728	37.644212
1886.409659	95673.352757	37.649229
1888.128883	95776.785408	37.654247
1890.062714	95878.511590	37.659264
1892.075037	95971.251204	37.664282
1893.775046	96068.780806	37.669300
1895.764415	96146.680880	37.674317
1897.050300	96239.103975	37.679335
1898.870593	96330.822586	37.684352
1900.949944	96425.999557	37.689370
1902.492636	96536.345517	37.694388
1903.874167	96622.632150	37.699405
1905.851203	96734.457344	37.704423
1907.691433	96850.741071	37.709440
1909.611019	96963.653560	37.714458
1911.165446	97087.335201	37.719476
1913.467633	97194.826506	37.724493
1915.449598	97305.182479	37.729511
1916.685880	97425.023524	37.734528
1918.849673	97549.283479	37.739546
1920.430334	97676.728282	37.744564
1922.862762	97804.382586	37.749581
1924.958222	97929.111085	37.754599
1926.932471	98052.540648	37.759616
1929.525577	98167.481750	37.764634
1931.412574	98292.928848	37.769652
1933.653367	98401.574778	37.774669
1935.340953	98527.256833	37.779687
1937.662337	98642.216814	37.784704
1939.990939	98745.817377	37.789722
1942.008181	98854.322350	37.794740
1944.047419	98961.163536	37.799757
1945.898888	99072.078502	37.804775
1947.901618	99188.155196	37.809792
1950.132094	99297.097364	37.814810
1952.333384	99407.502368	37.819828
1954.412149	99514.897019	37.824845
1956.463528	99625.757262	37.829863
1958.228005	99736.992396	37.834880
1960.422269	99834.012515	37.839898
1962.074347	99938.825738	37.844916
1963.591779	100049.301917	37.849933
1965.554635	100168.671894	37.854951
1967.482216	100282.685153	37.859968
1969.692968	100402.600379	37.864986
1971.443807	100521.066675	37.870004
1973.287645	100650.345749	37.875021
1975.050789	100777.064347	37.880039
1976.854022	100904.766046	37.885056
1979.167028	101022.347494	37.890074
1980.900221	101147.360687	37.895092
1982.619787	101268.154682	37.900109
1984.545344	101406.400071	37.905127
1986.615137	101532.414357	37.910144
1988.888217	101669.224554	37.915162
1990.467729	101806.143847	37.920180
1992.527872	101943.812599	37.925197
1994.526216	102075.215780	37.930215
1996.415274	102208.576393	37.935232
1998.519250	102334.664483	37.940250
2000.452792	102469.337758	37.945268
2002.179218	102612.576703	37.950285
2004.346476	102747.747046	37.955303
2006.121014	102882.015807	37.960320
2008.232943	103024.777820	37.965338
2010.314576	103178.537742	37.970356
2012.364255	103317.266205	37.975373
2014.287789	103445.035018	37.980391
2016.119472	103600.294080	37.985408
2018.121121	103734.201098	37.990426
2020.250131	103873.705569	37.995444
2022.081210	104011.723062	38.000461
2024.193106	104136.764395	38.005479
2026.128631	104253.300657	38.010496
2028.252039	104366.194329	38.015514
2029.709138	104502.966398	38.020532
2031.710884	104625.731831	38.025549
2033.501965	104763.238824	38.030567
2035.611742	104910.459725	38.035584
2037.501073	105039.317738	38.040602
2038.984146	105173.058055	38.045620
2041.188711	105329.395264	38.050637
2042.655596	105480.459741	38.055655
2044.708891	105640.258257	38.060672
2046.720958	105788.880370	38.065690
2048.816914	105964.029008	38.070708
2050.615010	106126.240881	38.075725
2052.864639	106276.894791	38.080743
2054.868219	106446.975686	38.085760
2057.083797	106610.138947	38.090778
2059.402616	106785.751463	38.095796
2061.424069	106942.669988	38.100813
2063.718926	107110.185237	38.105831
2065.612068	107278.157250	38.110848
2067.894915	107435.252696	38.115866
2069.888460	107612.327865	38.120884
2071.965726	107779.157630	38.125901
2074.261806	107941.883485	38.130919
2076.507014	108125.236858	38.135936
2078.815333	108298.132388	38.140954
2080.383931	108455.318867	38.145972
2082.874531	108630.749058	38.150989
2085.527871	108796.390353	38.156007
2087.329867	108963.142076	38.161024
2089.536526	109121.994393	38.166042
2092.116550	109287.636813	38.171060
2094.316624	109461.493460	38.176077
2096.337327	109618.043790	38.181095
2098.134774	109794.526693	38.186112
2100.288738	109950.626493	38.191130
2102.550142	110132.415393	38.196148
2104.953425	110294.336523	38.201165
2107.346787	110448.524217	38.206183
2109.193308	110620.336776	38.211200
2111.521975	110777.922014	38.216218
2113.630490	110942.732923	38.221236
2115.464523	111102.070978	38.226253
2117.746950	111258.574955	38.231271
2120.230471	111433.563697	38.236288
2122.074586	111582.363685	38.241306
2124.565495	111747.435543	38.246324
2126.151261	111903.417251	38.251341
2128.907695	112076.083676	38.256359
2130.552262	112242.368214	38.261376
2132.634235	112402.801993	38.266394
2134.947077	112580.067801	38.271412
2136.404617	112747.791672	38.276429
2138.810625	112915.887905	38.281447
2140.947845	113084.775240	38.286464
2142.909268	113255.466422	38.291482
2144.855113	113430.143176	38.296500
2146.721995	113612.049549	38.301517
2149.237023	113780.906383	38.306535
2151.546676	113955.439963	38.311552
2153.504852	114129.813761	38.316570
2155.920610	114307.338254	38.321588
2157.741400	114480.568395	38.326605
2160.574789	114649.227243	38.331623
2162.500360	114826.361674	38.336640
2164.609466	114982.883535	38.341658
2166.217716	115137.746829	38.346676
2168.564578	115298.304132	38.351693
2170.635049	115449.291449	38.356711
2172.320558	115608.266696	38.361728
2174.727415	115763.882820	38.366746
2176.553811	115924.093036	38.371764
2177.891122	116097.482516	38.376781
2180.444634	116256.261320	38.381799
2181.947111	116439.773398	38.386816
2184.186543	116611.235739	38.391834
2185.894098	116806.272363	38.396852
2188.081365	117001.805721	38.401869
2190.290883	117199.543612	38.406887
2192.227144	117392.175615	38.411904
2194.506013	117583.068030	38.416922
2196.819152	117787.122114	38.421940
2198.891671	118003.734193	38.426957
2201.300041	118208.384490	38.431975
2203.379395	118405.375325	38.436992
2205.590723	118618.417600	38.442010
2207.839923	118828.347459	38.447028
2209.965919	119045.388378	38.452045
2212.965285	119253.427381	38.457063
2214.840732	119462.721547	38.462080
2217.300741	119682.441014	38.467098
2219.629730	119888.609530	38.472116
2221.828124	120101.535229	38.477133
2224.206048	120305.427730	38.482151
2226.253136	120528.121459	38.487168
2228.747702	120731.731572	38.492186
2231.037126	120943.848502	38.497204
2233.133247	121171.891366	38.502221
2235.878715	121385.042961	38.507239
2237.280575	121605.598504	38.512256
2239.611852	121826.250904	38.517274
2241.999880	122059.200573	38.522292
2244.279802	122276.806337	38.527309
2246.418899	122492.215350	38.532327
2249.186807	122726.111690	38.537344
2251.269579	122947.976327	38.542362
2253.409909	123171.012980	38.547380
2255.491365	123399.489659	38.552397
2257.634684	123615.779434	38.557415
2260.507396	123851.708437	38.562432
2262.499598	124080.799217	38.567450
2264.600214	124306.157289	38.572468
2266.757050	124543.153815	38.577485
2269.633563	124760.946210	38.582503
2271.865839	124995.840345	38.587520
2274.607555	125212.831645	38.592538
2277.119911	125437.421166	38.597556
2279.547631	125660.629640	38.602573
2281.891581	125878.130749	38.607591
2283.741643	126094.593846	38.612608
2285.814176	126316.072634	38.617626
2288.268537	126534.194293	38.622644
2290.480622	126758.470120	38.627661
2292.880485	126973.760754	38.632679
2295.394671	127202.508310	38.637696
2297.386600	127422.064521	38.642714
2299.654065	127652.489798	38.647732
2301.863095	127878.814808	38.652749
2303.851365	128099.770767	38.657767
2306.101326	128340.720404	38.662784
2307.981779	128569.054416	38.667802
2310.732752	128802.696450	38.672820
2312.870453	129038.795623	38.677837
2315.017361	129260.417996	38.682855
2317.365316	129477.683546	38.687872
2319.520260	129700.626492	38.692890
2321.615791	129898.927305	38.697908
2323.781053	130119.916896	38.702925
2326.209474	130332.949131	38.707943
2328.402501	130555.141990	38.712960
2330.466925	130780.832674	38.717978
2332.960263	131002.968180	38.722996
2334.950662	131226.794923	38.728013
2336.990118	131448.521571	38.733031
2339.196553	131701.208366	38.738048
2342.059052	131932.731085	38.743066
2344.565039	132163.587561	38.748084
2347.279757	132393.384825	38.753101
2349.390645	132628.581633	38.758119
2351.590188	132870.693900	38.763136
2353.889139	133124.161148	38.768154
2356.551090	133357.714918	38.773172
2358.745268	133598.613883	38.778189
2360.630130	133858.075865	38.783207
2363.158302	134106.005823	38.788224
2365.311544	134357.155420	38.793242
2367.790721	134615.856308	38.798260
2370.146869	134879.844011	38.803277
2371.891450	135132.990659	38.808295
2374.434020	135406.037900	38.813312
2376.800706	135685.865150	38.818330
2379.326777	135950.961897	38.823348
2381.374961	136231.844813	38.828365
2383.897974	136508.366025	38.833383
2386.392974	136785.629299	38.838400
2388.541910	137065.372162	38.843418
2391.595215	137355.216098	38.848436
2393.685223	137647.852084	38.853453
2396.225074	137923.021300	38.858471
2398.873564	138195.040654	38.863488
2401.420313	138476.874443	38.868506
2404.115382	138752.747613	38.873524
2406.669145	139041.017728	38.878541
2408.970961	139319.049663	38.883559
2411.536693	139594.757631	38.888576
2413.725751	139873.102338	38.893594
2416.386125	140147.783450	38.898612
2418.874606	140433.305638	38.903629
2421.014444	140699.974581	38.908647
2423.506248	140991.083572	38.913664
2425.869908	141272.124957	38.918682
2428.313123	141551.112251	38.923700
2431.041186	141844.359597	38.928717
2433.388818	142115.255384	38.933735
2436.020530	142398.926513	38.938752
2438.219107	142690.802250	38.943770
2440.479702	142973.747877	38.948788
2442.819927	143264.881433	38.953805
2444.880742	143562.101637	38.958823
2447.557205	143859.531909	38.963840
2450.108173	144146.766671	38.968858
2452.653154	144433.496338	38.973876
2454.535088	144726.639261	38.978893
2457.184207	145024.524923	38.983911
2459.505137	145320.483703	38.988928
2461.695825	145619.168012	38.993946
2464.321601	145931.493645	38.998964
2466.473913	146238.259844	39.003981
2468.829837	146539.297126	39.008999
2471.624231	146851.145032	39.014016
2473.404147	147161.820783	39.019034
2475.975337	147452.992955	39.024052
2477.857574	147746.432277	39.029069
2480.348064	148048.574184	39.034087
2482.808759	148335.960703	39.039104
2484.801517	148639.516596	39.044122
2487.435449	148937.033608	39.049140
2489.362293	149241.859850	39.054157
2491.770800	149561.603074	39.059175
2494.176610	149863.006932	39.064192
2496.484914	150197.671429	39.069210
2498.716599	150515.163164	39.074228
2501.527177	150849.600785	39.079245
2503.854036	151180.650786	39.084263
2506.210391	151505.554469	39.089280
2508.505297	151851.299979	39.094298
2511.216461	152187.119491	39.099316
2513.899182	152539.663240	39.104333
2516.031906	152885.440532	39.109351
2518.619836	153223.900481	39.114368
2521.110958	153584.262151	39.119386
2523.891406	153927.266046	39.124404
2526.416110	154294.164433	39.129421
2529.250740	154641.899078	39.134439
2532.087742	154995.792218	39.139456
2535.022248	155335.644904	39.144474
2538.000664	155687.298608	39.149492
2540.597129	156037.846267	39.154509
2543.183301	156384.386108	39.159527
2545.461614	156735.228874	39.164544
2548.069632	157097.498255	39.169562
2550.699580	157454.929646	39.174580
2553.339472	157811.587214	39.179597
2555.482293	158171.396841	39.184615
2557.875295	158537.682064	39.189632
2559.959740	158910.479605	39.194650
2562.764253	159272.274227	39.199668
2565.042396	159642.544931	39.204685
2567.586625	160019.974529	39.209703
2570.512222	160396.051812	39.214720
2572.821066	160788.211557	39.219738
2575.911678	161163.366223	39.224756
2578.391202	161539.786696	39.229773
2581.043300	161916.525176	39.234791
2583.833514	162288.064340	39.239808
2586.643919	162670.381344	39.244826
2589.128254	163047.850928	39.249844
2591.579283	163440.055377	39.254861
2594.063321	163827.775243	39.259879
2596.628890	164205.733900	39.264896
2599.095086	164599.834572	39.269914
2601.514999	164980.080327	39.274932
2603.881467	165380.701718	39.279949
2606.755563	165773.894765	39.284967
2609.034037	166167.957726	39.289984
2611.571675	166576.215391	39.295002
2614.051878	166969.540346	39.300020
2616.921111	167374.500448	39.305037
2618.988663	167787.181026	39.310055
2621.454850	168192.285037	39.315072
2623.951291	168613.143659	39.320090
2626.232156	169031.422851	39.325108
2629.284494	169453.265977	39.330125
2631.653235	169880.360859	39.335143
2634.441866	170304.192809	39.340160
2637.012871	170718.284204	39.345178
2639.895511	171143.896565	39.350196
2641.998925	171564.173257	39.355213
2644.651319	171998.409992	39.360231
2647.161097	172406.209476	39.365248
2649.546229	172829.559987	39.370266
2652.381350	173225.897602	39.375284
2654.701714	173636.031470	39.380301
2656.748826	174047.149856	39.385319
2659.525012	174463.718068	39.390336
2661.673539	174886.888042	39.395354
2664.255757	175307.021021	39.400372
2666.906238	175750.053100	39.405389
2669.238025	176181.010528	39.410407
2671.695361	176612.953725	39.415424
2674.311301	177074.182326	39.420442
2677.152888	177529.359056	39.425460
2679.827237	177970.062599	39.430477
2682.109577	178443.947752	39.435495
2684.855454	178900.238766	39.440512
2687.276414	179378.501045	39.445530
2690.295095	179843.668796	39.450548
2692.441494	180328.988863	39.455565
2694.959289	180806.938825	39.460583
2698.064606	181283.580275	39.465600
2701.259697	181778.268262	39.470618
2703.816802	182252.333593	39.475636
2706.590894	182742.927157	39.480653
2709.073948	183304.608663	39.485671
2711.750838	183803.528163	39.490688
2714.403807	184298.390113	39.495706
2717.742882	184801.071699	39.500724
2720.415525	185300.939125	39.505741
2723.138029	185805.119072	39.510759
2726.183630	186296.449657	39.515776
2728.656941	186807.988455	39.520794
2731.172003	187305.401002	39.525812
2734.074571	187819.696863	39.530829
2736.842899	188323.602207	39.535847
2739.403736	188836.254490	39.540864
2741.814736	189362.750198	39.545882
2745.009063	189890.802243	39.550900
2747.957042	190405.687070	39.555917
2750.180662	190938.086744	39.560935
2752.886882	191459.262484	39.565952
2755.301455	191998.037936	39.570970
2758.169672	192535.017550	39.575988
2760.806459	193080.062348	39.581005
2763.617510	193627.571527	39.586023
2766.394061	194161.854460	39.591040
2769.085295	194717.820125	39.596058
2772.136640	195251.175431	39.601076
2775.066244	195801.088176	39.606093
2777.509148	196349.656739	39.611111
2780.525892	196899.636378	39.616128
2783.602835	197448.033798	39.621146
2786.374448	197998.868789	39.626164
2789.471542	198536.623740	39.631181
2792.262780	199086.519752	39.636199
2795.041474	199632.990388	39.641216
2797.662423	200179.589178	39.646234
2800.539073	200734.837372	39.651252
2803.237063	201291.309267	39.656269
2805.515940	201842.844257	39.661287
2808.646149	202395.619580	39.666304
2811.238342	202961.994910	39.671322
2814.000617	203518.489175	39.676340
2816.876804	204086.449291	39.681357
2819.747875	204655.199366	39.686375
2822.578139	205218.114802	39.691392
2825.384964	205771.661785	39.696410
2828.107858	206335.409949	39.701428
2831.112967	206876.532147	39.706445
2834.121208	207424.488606	39.711463
2836.965937	207946.789356	39.716480
2839.569108	208474.692344	39.721498
2842.246471	208995.573571	39.726516
2845.275389	209534.615080	39.731533
2847.822736	210054.782106	39.736551
2850.610787	210596.378386	39.741568
2852.932331	211147.879820	39.746586
2855.655472	211692.892408	39.751604
2859.081584	212233.782280	39.756621
2861.560690	212778.123659	39.761639
2864.889405	213320.707239	39.766656
2867.708065	213872.694600	39.771674
2870.108112	214437.551755	39.776692
2872.961698	214989.205081	39.781709
2875.090404	215575.851950	39.786727
2877.924295	216155.784354	39.791744
2880.825603	216742.286564	39.796762
2883.316971	217335.534826	39.801780
2886.622093	217939.097520	39.806797
2888.717981	218541.427357	39.811815
2891.604055	219152.678028	39.816832
2894.186971	219770.353070	39.821850
2896.878266	220382.905469	39.826868
2900.237857	221007.217484	39.831885
2902.577016	221644.442321	39.836903
2905.421590	222275.847158	39.841920
2907.884965	222927.508137	39.846938
2910.739006	223576.567855	39.851956
2913.559457	224235.667613	39.856973
2916.378985	224901.042434	39.861991
2919.104854	225576.060089	39.867008
2922.582247	226236.149598	39.872026
2925.444174	226922.806304	39.877044
2928.495156	227602.599558	39.882061
2931.282411	228280.096615	39.887079
2934.352092	228954.780123	39.892096
2937.476468	229637.253703	39.897114
2940.718508	230319.530555	39.902132
2943.752976	231003.388933	39.907149
2946.634215	231684.196736	39.912167
2949.776637	232365.699679	39.917184
2952.658267	233051.993126	39.922202
2955.590376	233736.296279	39.927220
2958.898605	234419.548891	39.932237
2961.979737	235107.840515	39.937255
2965.414111	235789.699417	39.942272
2969.003940	236461.752385	39.947290
2972.429698	237126.411906	39.952308
2975.676004	237788.405424	39.957325
2978.561556	238452.079840	39.962343
2982.272242	239108.460012	39.967360
2985.613408	239763.245285	39.972378
2988.217279	240425.028648	39.977396
2991.508006	241072.477120	39.982413
2993.950296	241727.093346	39.987431
2997.117089	242383.194946	39.992448
3000.450014	243028.116797	39.997466
3003.262499	243686.912071	40.002484
3006.391177	244323.275936	40.007501
3009.175273	244985.247092	40.012519
3012.015681	245635.318816	40.017536
3015.560929	246290.790599	40.022554
3018.101811	246946.696658	40.027572
3021.362031	247598.118707	40.032589
3024.193343	248257.226239	40.037607
3026.837436	248910.848291	40.042624
3030.148146	249557.911453	40.047642
3032.899820	250193.501563	40.052660
3035.164578	250809.554961	40.057677
3038.593519	251434.771855	40.062695
3041.483426	252064.871484	40.067712
3044.087142	252686.097246	40.072730
3046.951896	253331.106335	40.077748
3049.694202	253977.274778	40.082765
3052.498046	254627.139268	40.087783
3054.959793	255293.133228	40.092800
3058.080344	255946.675943	40.097818
3060.554337	256623.914110	40.102836
3064.123337	257301.460141	40.107853
3066.813674	257981.807047	40.112871
3070.001280	258663.063109	40.117888
3073.014930	259342.615342	40.122906
3075.996403	260042.362013	40.127924
3078.974079	260743.730717	40.132941
3082.015423	261456.718396	40.137959
3084.732371	262160.760747	40.142976
3087.947239	262877.522201	40.147994
3090.161603	263609.675080	40.153012
3093.626622	264345.335663	40.158029
3096.036628	265091.671287	40.163047
3098.977575	265842.871252	40.168064
3102.062940	266602.170634	40.173082
3104.802564	267358.698998	40.178100
3108.118315	268140.021778	40.183117
3110.913468	268911.539666	40.188135
3113.584626	269707.198631	40.193152
3116.743745	270500.920367	40.198170
3119.718723	271299.337055	40.203188
3123.091770	272103.779652	40.208205
3126.033927	272911.634608	40.213223
3129.326154	273713.027216	40.218240
3132.812426	274524.032544	40.223258
3135.801758	275342.904299	40.228276
3139.809563	276157.164266	40.233293
3142.548932	276975.296692	40.238311
3145.857797	277778.754565	40.243328
3149.313431	278610.014368	40.248346
3152.133241	279438.596508	40.253364
3155.454888	280250.711496	40.258381
3158.430025	281084.863331	40.263399
3161.587890	281911.358844	40.268416
3164.720241	282742.115026	40.273434
3167.854961	283576.060699	40.278452
3171.253828	284407.111092	40.283469
3174.491204	285241.757124	40.288487
3177.779721	286080.168415	40.293504
3181.501291	286907.862155	40.298522
3184.481747	287743.558323	40.303540
3188.193146	288565.824294	40.308557
3191.977900	289382.202912	40.313575
3195.537866	290193.299488	40.318592
3199.612054	291011.186054	40.323610
3202.827960	291815.129805	40.328628
3206.052197	292616.421152	40.333645
3209.246438	293418.772953	40.338663
3212.631622	294226.669788	40.343680
3216.000114	295020.314995	40.348698
3219.256624	295813.992328	40.353716
3222.451446	296608.709329	40.358733
3225.387654	297402.287875	40.363751
3228.533260	298206.206048	40.368768
3231.684088	298993.711729	40.373786
3234.681115	299798.848695	40.378804
3238.056569	300605.463217	40.383821
3241.139461	301388.477041	40.388839
3244.049202	302168.739453	40.393856
3247.010128	302915.346823	40.398874
3250.274807	303686.011803	40.403892
3253.506946	304451.517376	40.408909
3256.297929	305227.361148	40.413927
3259.869463	305995.303624	40.418944
3262.889707	306770.605663	40.423962
3265.832899	307566.341067	40.428980
3269.307503	308348.705493	40.433997
3272.337671	309130.543142	40.439015
3275.253665	309934.950484	40.444032
3278.487174	310730.766602	40.449050
3281.259111	311548.976835	40.454068
3284.483410	312365.173253	40.459085
3287.372056	313197.752662	40.464103
3290.508930	314031.775702	40.469120
3293.861885	314878.566259	40.474138
3296.614720	315732.870819	40.479156
3299.843849	316582.542022	40.484173
3303.029158	317447.861916	40.489191
3305.758273	318321.230002	40.494208
3308.981528	319207.318616	40.499226
3312.012300	320109.228541	40.504244
3314.988227	321007.981538	40.509261
3318.029430	321915.307486	40.514279
3321.278812	322832.147537	40.519296
3324.544856	323746.199096	40.524314
3327.740350	324680.692408	40.529332
3331.147785	325614.598444	40.534349
3334.848246	326554.348897	40.539367
3338.433092	327482.170822	40.544384
3342.677754	328423.542941	40.549402
3345.861133	329363.815392	40.554420
3349.338589	330296.560557	40.559437
3352.347234	331240.671222	40.564455
3355.915992	332191.825045	40.569472
3359.950033	333127.687000	40.574490
3363.177533	334075.954969	40.579508
3367.050398	335006.848712	40.584525
3370.449471	335944.236127	40.589543
3373.718311	336902.343481	40.594560
3377.032347	337837.108482	40.599578
3380.451342	338781.978509	40.604596
3383.941960	339719.330258	40.609613
3387.932204	340672.785919	40.614631
3391.211454	341613.341634	40.619648
3395.016369	342557.061478	40.624666
3398.639649	343506.084410	40.629684
3402.258447	344434.667159	40.634701
3405.947487	345361.996429	40.639719
3409.479066	346294.066971	40.644736
3412.989997	347221.499776	40.649754
3415.969139	348152.083502	40.654772
3419.382324	349084.018524	40.659789
3422.957439	350015.622880	40.664807
3426.315817	350955.728400	40.669824
3429.814335	351893.883134	40.674842
3433.100772	352825.122129	40.679860
3436.271949	353761.828125	40.684877
3439.824339	354706.534068	40.689895
3442.756899	355654.705559	40.694912
3446.142943	356595.020102	40.699930
3449.234933	357546.252394	40.704948
3452.908088	358502.104619	40.709965
3456.397266	359457.398000	40.714983
3459.642279	360403.802544	40.720000
3462.970493	361362.178512	40.725018
3465.960399	362313.988372	40.730023
3469.524939	363228.294685	40.735028
3472.589533	364101.717057	40.740032
3475.524827	364925.231941	40.745037
3478.919268	365698.878460	40.750042
3481.793464	366419.866400	40.755047
3484.927641	367078.702718	40.760052
3487.625597	367693.767196	40.765056
3490.007953	368244.363877	40.770061
3492.763877	368747.130489	40.775066
3495.255702	369202.728128	40.780071
3497.405686	369616.658475	40.785076
3499.637054	369969.880625	40.790080
3501.827758	370276.311614	40.795085
3503.847072	370541.054042	40.800090
3505.287707	370767.779986	40.805095
3506.632212	370934.797135	40.810100
3508.689407	371075.918136	40.815104
3510.078327	371185.542082	40.820109
3511.313585	371262.445779	40.825114
3512.466983	371293.815418	40.830119
3513.612142	371306.794916	40.835124
3515.146754	371296.876688	40.840128
3515.370693	371258.407712	40.845133
3516.318959	371195.210349	40.850138
3516.881548	371109.007526	40.855143
3517.431250	371004.110025	40.860148
3518.323094	370883.739104	40.865152
3518.624057	370748.777113	40.870157
3519.418294	370595.167670	40.875162
3519.809227	370431.992594	40.880167
3520.160989	370253.860067	40.885172
3520.701840	370058.549410	40.890176
3520.937357	369857.416853	40.895181
3520.969217	369644.171590	40.900186
3521.132150	369419.040462	40.905191
3521.301044	369195.938959	40.910196
3521.484454	368948.165548	40.915200
3521.569465	368711.456456	40.920205
3521.961359	368452.188532	40.925210
3522.164576	368204.913631	40.930215
3522.298792	367950.889503	40.935220
3522.632701	367673.306168	40.940224
3522.251419	367403.021843	40.945229
3522.324060	367130.885563	40.950234
3522.197311	366861.648803	40.955239
3522.225600	366582.298812	40.960244
3522.262056	366307.543495	40.965248
3522.063253	366035.922017	40.970253
3522.102098	365745.052797	40.975258
3522.209470	365466.238604	40.980263
3521.808980	365185.544716	40.985268
3521.991391	364898.786061	40.990272
3521.758657	364612.191119	40.995277
3521.586556	364316.817879	41.000282
3521.127388	364043.617736	41.005287
3521.641579	363759.489379	41.010292
3521.345747	363473.528382	41.015296
3520.781564	363199.345832	41.020301
3521.260519	362918.543533	41.025306
3520.778719	362635.678083	41.030311
3520.859923	362357.753171	41.035316
3520.952351	362066.102154	41.040320
3520.711123	361791.271628	41.045325
3520.664778	361509.470862	41.050330
3520.440148	361237.199158	41.055335
3520.561761	360943.855455	41.060340
3520.315578	360671.963155	41.065344
3519.738540	360400.831656	41.070349
3519.844108	360125.626680	41.075354
3519.627523	359860.812455	41.080359
3519.732944	359589.389080	41.085364
3519.265498	359321.432758	41.090368
3519.153260	359041.499746	41.095373
3519.070518	358783.669231	41.100378
3519.005308	358520.420688	41.105383
3518.643380	358254.192013	41.110388
3518.976142	357989.351847	41.115392
3518.727536	357736.265445	41.120397
3518.754018	357469.257630	41.125402
3518.436763	357206.113447	41.130407
3518.462935	356958.035217	41.135412
3518.273766	356700.305493	41.140416
3518.025673	356445.327692	41.145421
3517.922758	356181.632975	41.150426
3517.554425	355933.455725	41.155431
3517.391895	355692.208298	41.160436
3517.420118	355445.261379	41.165440
3516.968302	355204.487485	41.170445
3517.220109	354948.961794	41.175450
3517.037046	354726.111721	41.180455
3516.861247	354484.374146	41.185460
3516.888184	354238.256687	41.190464
3516.100249	354004.439609	41.195469
3516.041622	353768.142953	41.200474
3516.195353	353545.714823	41.205479
3516.086961	353318.267953	41.210484
3516.178746	353090.686489	41.215488
3516.084151	352862.675008	41.220493
3516.203904	352637.576924	41.225498
3515.957244	352419.855097	41.230503
3515.726069	352194.707085	41.235508
3515.592972	351964.356691	41.240512
3515.149308	351746.533995	41.245517
3515.325335	351527.469075	41.250522
3515.522157	351313.025761	41.255527
3515.086766	351089.122074	41.260532
3515.338869	350873.980875	41.265536
3514.581108	350672.265359	41.270541
3514.640495	350461.523789	41.275546
3514.149235	350245.604934	41.280551
3513.935604	350038.563832	41.285556
3514.026358	349839.201702	41.290560
3513.624061	349652.880036	41.295565
3513.988749	349441.880783	41.300570
3513.775018	349255.095218	41.305575
3513.566601	349051.580587	41.310580
3513.701141	348856.196768	41.315584
3513.186740	348668.260070	41.320589
3513.243246	348477.233288	41.325594
3513.106652	348290.506457	41.330599
3512.957974	348102.661896	41.335604
3513.166600	347910.819981	41.340608
3512.610973	347736.459842	41.345613
3512.778540	347544.774767	41.350618
3512.704586	347371.405152	41.355623
3512.675275	347184.604487	41.360628
3512.808411	347004.234776	41.365632
3512.308918	346836.191430	41.370637
3512.336020	346649.912841	41.375642
3512.426029	346477.326496	41.380647
3512.126666	346299.639199	41.385652
3512.348586	346117.827134	41.390656
3512.097214	345953.147326	41.395661
3512.087570	345773.225528	41.400666
3511.738521	345610.338980	41.405671
3511.413912	345441.295220	41.410676
3511.412239	345271.589951	41.415680
3511.345448	345116.157013	41.420685
3511.408130	344948.524856	41.425690
3510.968426	344791.699545	41.430695
3511.032157	344628.947150	41.435700
3511.016966	344473.198114	41.440704
3510.849351	344311.904159	41.445709
3510.436492	344152.834330	41.450714
3510.526434	344010.897924	41.455719
3510.272718	343859.632770	41.460724
3510.693013	343695.218405	41.465728
3510.753647	343554.352557	41.470733
3510.490780	343412.672241	41.475738
3510.324455	343264.492719	41.480743
3510.331406	343115.904085	41.485748
3510.230642	342963.899166	41.490752
3510.089525	342829.825172	41.495757
3509.756894	342682.940453	41.500762
3509.979451	342537.341328	41.505767
3509.654041	342405.659137	41.510772
3509.658307	342249.363057	41.515776
3509.271866	342124.656164	41.520781
3509.517228	341989.247183	41.525786
3509.428199	341860.856853	41.530791
3509.466366	341718.715729	41.535796
3509.530135	341587.274725	41.540800
3509.247891	341461.684662	41.545805
3509.037516	341329.243044	41.550810
3509.066377	341199.611362	41.555815
3508.932079	341072.827130	41.560820
3508.888421	340941.756483	41.565824
3508.600674	340827.175032	41.570829
3508.380137	340704.598474	41.575834
3508.472321	340587.820940	41.580839
3508.582686	340464.327278	41.585844
3508.478832	340337.688209	41.590848
3507.886833	340236.120550	41.595853
3508.190665	340111.934290	41.600858
3508.096526	339998.998127	41.605863
3507.905036	339882.847460	41.610868
3508.163649	339766.270052	41.615872
3507.671076	339657.667023	41.620877
3507.865806	339544.175689	41.625882
3507.744898	339441.184407	41.630887
3507.621037	339331.022464	41.635892
3507.633740	339221.499973	41.640896
3507.204026	339124.938618	41.645901
3507.220065	339015.720119	41.650906
3507.653957	338909.538269	41.655911
3507.337425	338808.940623	41.660916
3507.411814	338704.212955	41.665920
3507.002334	338607.291036	41.670925
3506.944113	338500.116894	41.675930
3506.770038	338401.453872	41.680935
3507.024763	338308.343392	41.685940
3507.233582	338205.907312	41.690944
3506.831148	338125.410290	41.695949
3506.959095	338026.037861	41.700954
3506.618933	337934.341747	41.705959
3506.368622	337837.316585	41.710964
3506.826934	337741.579005	41.715968
3506.709701	337648.677554	41.720973
3506.485279	337551.316992	41.725978
3506.469498	337461.272758	41.730983
3506.217127	337370.985560	41.735988
3506.421026	337284.492151	41.740992
3506.481226	337202.038936	41.745997
3506.293598	337106.070077	41.751002
3506.029868	337021.937854	41.756007
3506.151101	336948.197042	41.761012
3506.266482	336860.877271	41.766016
3505.825158	336788.419304	41.771021
3505.822225	336697.964289	41.776026
3505.746253	336613.216874	41.781031
3506.145645	336535.922351	41.786036
3505.897852	336445.199828	41.791040
3505.903698	336372.060794	41.796045
3505.894575	336291.371069	41.801050
3506.015679	336210.915113	41.806055
3505.449955	336142.264481	41.811060
3505.953140	336057.908421	41.816064
3505.594747	335986.987178	41.821069
3505.527034	335908.391098	41.826074
3505.556355	335831.025794	41.831079
3505.500989	335764.354572	41.836084
3505.636845	335682.293004	41.841088
3505.492733	335609.150466	41.846093
3505.530962	335527.917612	41.851098
3505.418865	335463.111187	41.856103
3505.267822	335388.138251	41.861108
3505.590063	335317.795955	41.866112
3504.912810	335239.420901	41.871117
3504.764117	335171.084732	41.876122
3505.000456	335118.226832	41.881127
3505.206189	335053.344569	41.886132
3505.053811	334981.041320	41.891136
3504.844348	334908.695991	41.896141
3505.071224	334837.274138	41.901146
3504.706678	334781.279887	41.906151
3504.780327	334716.392254	41.911156
3504.855733	334645.375188	41.916160
3504.799485	334594.418802	41.921165
3504.931775	334527.334541	41.926170
3504.781550	334454.216114	41.931175
3504.863479	334394.565588	41.936180
3505.013594	334324.960419	41.941184
3504.705499	334264.175359	41.946189
3504.488697	334199.535692	41.951194
3504.611982	334146.973842	41.956199
3504.253158	334094.360129	41.961204
3504.468552	334031.076800	41.966208
3504.322473	333983.668693	41.971213
3504.523596	333926.262250	41.976218
3504.188032	333855.028178	41.981223
3504.368424	333807.695971	41.986228
3504.759549	333750.412149	41.991232
3504.231031	333691.059397	41.996237
3504.643491	333636.442465	42.001242
3504.309151	333575.838419	42.006247
3504.050065	333524.276477	42.011252
3503.933674	333465.443885	42.016256
3503.919848	333418.573905	42.021261
3504.287150	333367.956555	42.026266
3504.035930	333308.508982	42.031271
3503.591727	333262.748830	42.036276
3503.963166	333204.729709	42.041280
3503.776208	333169.331200	42.046285
3503.850613	333119.496857	42.051290
3503.809078	333081.837449	42.056295
3503.477299	333023.088706	42.061300
3503.576977	332973.275652	42.066304
3503.625230	332937.382362	42.071309
3503.789526	332889.110501	42.076314
3503.470371	332850.451515	42.081319
3503.384565	332798.454564	42.086324
3503.594735	332764.799331	42.091328
3503.221778	332716.916440	42.096333
3503.577720	332675.939059	42.101338
3503.383842	332631.715856	42.106343
3503.109743	332598.848313	42.111348
3503.441873	332557.543896	42.116352
3503.210816	332517.929771	42.121357
3503.348572	332466.940174	42.126362
3503.489539	332426.962594	42.131367
3503.271365	332389.482712	42.136372
3503.399433	332343.047015	42.141376
3503.258093	332306.216305	42.146381
3503.207470	332269.295076	42.151386
3503.356746	332229.265123	42.156391
3503.237093	332193.524547	42.161396
3503.159246	332146.535835	42.166400
3503.141643	332107.218545	42.171405
3503.488022	332079.263936	42.176410
3503.501852	332032.006415	42.181415
3503.221758	331997.180910	42.186420
3503.232193	331962.818624	42.191424
3502.974907	331924.225323	42.196429
3503.312680	331880.350501	42.201434
3503.188973	331843.999825	42.206439
3503.176533	331806.563507	42.211444
3502.887917	331763.498621	42.216448
3502.729910	331742.566011	42.221453
3503.289805	331699.088627	42.226458
3503.541332	331669.902296	42.231463
3503.132266	331636.698951	42.236468
3503.384758	331586.402385	42.241472
3503.255107	331551.476652	42.246477
3503.177425	331510.260606	42.251482
3503.031214	331467.478330	42.256487
3502.988971	331432.106448	42.261492
3503.200953	331393.083173	42.266496
3502.995298	331362.823557	42.271501
3503.113792	331332.920184	42.276506
3502.834009	331301.832788	42.281511
3502.663161	331269.965317	42.286516
3502.720058	331234.221677	42.291520
3502.530984	331207.418373	42.296525
3502.962108	331177.364266	42.301530
3502.635167	331140.332543	42.306535
3502.546017	331107.231328	42.311540
3502.453660	331083.159700	42.316544
3502.350452	331058.123256	42.321549
3502.705365	331026.173386	42.326554
3502.752302	330997.272871	42.331559
3502.668809	330977.269258	42.336564
3502.714691	330938.271490	42.341568
3502.818002	330908.217555	42.346573
3502.759003	330873.229293	42.351578
3502.702898	330853.373939	42.356583
3502.395816	330818.475280	42.361588
3502.706001	330788.795859	42.366592
3502.594884	330761.267896	42.371597
3502.587341	330720.141775	42.376602
3502.468465	330704.645434	42.381607
3502.457865	330684.452233	42.386612
3502.295260	330645.690239	42.391616
3502.195045	330640.822535	42.396621
3502.551755	330606.150556	42.401626
3502.471256	330584.518468	42.406631
3502.190699	330554.982092	42.411636
3502.667836	330527.056782	42.416640
3502.179059	330512.915352	42.421645
3502.293531	330477.975915	42.426650
3502.375263	330454.461671	42.431655
3502.271185	330432.909489	42.436660
3502.191336	330413.464574	42.441664
3502.343270	330383.809583	42.446669
3502.382171	330358.775904	42.451674
3502.214980	330343.134363	42.456679
3502.400874	330311.820759	42.461684
3502.469546	330280.423717	42.466688
3502.417132	330272.369163	42.471693
3502.352036	330245.215158	42.476698
3502.497414	330205.132839	42.481703
3502.052750	330195.181121	42.486708
3502.299461	330158.185946	42.491712
3502.292430	330148.292970	42.496717
3502.459935	330119.754472	42.501722
3502.238750	330094.405197	42.506727
3502.025237	330070.275575	42.511732
3502.445053	330041.036268	42.516736
3502.276055	330031.626411	42.521741
3502.112889	330006.191703	42.526746
3502.283999	329984.392770	42.531751
3502.222284	329968.785459	42.536756
3502.125028	329947.537158	42.541760
3501.817513	329931.815651	42.546765
3502.378519	329907.030709	42.551770
3502.231791	329878.363116	42.556775
3501.998240	329861.180226	42.561780
3502.263525	329832.371881	42.566784
3502.108785	329819.729507	42.571789
3502.299112	329790.881980	42.576794
3502.034182	329772.813734	42.581799
3501.895557	329756.709662	42.586804
3501.951145	329733.173635	42.591808
3501.619794	329720.660579	42.596813
3502.249226	329707.234261	42.601818
3502.357696	329687.784978	42.606823
3501.948497	329667.933350	42.611828
3502.481709	329647.298501	42.616832
3502.490122	329616.978617	42.621837
3502.263674	329593.435728	42.626842
3501.988730	329565.754484	42.631847
3502.254728	329554.699528	42.636852
3502.263569	329525.269736	42.641856
3502.006149	329515.720967	42.646861
3501.780567	329484.343852	42.651866
3502.294078	329465.619624	42.656871
3501.647382	329447.356560	42.661876
3502.194676	329424.710012	42.666880
3501.896220	329407.435329	42.671885
3501.804697	329389.543276	42.676890
3501.948664	329371.461788	42.681895
3501.845971	329359.345267	42.686900
3501.918990	329340.181141	42.691904
3502.163505	329327.628800	42.696909
3502.119738	329304.896541	42.701914
3502.075159	329290.761526	42.706919
3502.160057	329273.121627	42.711924
3501.832400	329251.476568	42.716928
3501.681302	329242.012851	42.721933
3501.848226	329218.993251	42.726938
3501.848277	329213.244891	42.731943
3502.033946	329177.148567	42.736948
3501.884047	329160.054032	42.741952
3501.919719	329144.965310	42.746957
3502.014432	329132.105666	42.751962
3501.882769	329118.645523	42.756967
3501.536904	329096.799742	42.761972
3501.724239	329076.549327	42.766976
3501.641857	329076.994645	42.771981
3501.732105	329047.780685	42.776986
3501.474686	329038.231799	42.781991
3501.711891	329031.581532	42.786996
3501.445186	329011.834470	42.792001
3501.381938	328997.549655	42.797005
3501.743660	328985.106058	42.802010
3501.750937	328977.983018	42.807015
3501.647579	328966.324319	42.812020
3502.076837	328947.841937	42.817025
3501.392694	328943.446844	42.822029
3502.277831	328922.527675	42.827034
3501.885961	328907.251347	42.832039
3502.327740	328887.266282	42.837044
3502.288313	328872.418115	42.842049
3501.805683	328849.474413	42.847053
3502.048866	328824.763911	42.852058
3501.848496	328816.198040	42.857063
3501.716875	328793.937062	42.862068
3501.958211	328775.534849	42.867073
3501.638943	328760.654084	42.872077
3501.681315	328734.779445	42.877082
3501.766049	328730.543915	42.882087
3501.501595	328721.988042	42.887092
3501.998240	328696.016922	42.892097
3501.657855	328691.110216	42.897101
3501.933318	328668.098760	42.902106
3501.911001	328651.289286	42.907111
3501.764738	328645.233054	42.912116
3501.689429	328628.915134	42.917121
3501.652524	328615.999591	42.922125
3501.626128	328602.115843	42.927130
3501.590831	328593.829345	42.932135
3501.380894	328578.244653	42.937140
3501.563644	328559.317348	42.942145
3501.690010	328564.232166	42.947149
3501.993556	328541.724962	42.952154
3501.495551	328527.736867	42.957159
3501.493958	328514.815771	42.962164
3501.651561	328507.821759	42.967169
3501.649308	328493.603532	42.972173
3502.029682	328476.985387	42.977178
3501.657083	328467.632420	42.982183
3501.636800	328443.268099	42.987188
3502.107215	328424.422936	42.992193
3501.657030	328424.645968	42.997197
3501.728662	328408.254112	43.002202
3501.816039	328391.758045	43.007207
3501.588739	328391.717309	43.012212
3502.014172	328359.957722	43.017217
3501.501954	328356.960093	43.022221
3501.540254	328341.845216	43.027226
3501.748241	328320.395697	43.032231
3501.569101	328323.425178	43.037236
3501.693462	328301.836107	43.042241
3501.555381	328280.288055	43.047245
3501.755385	328263.469094	43.052250
3501.773935	328259.956068	43.057255
3501.566546	328243.633202	43.062260
3502.023473	328222.119275	43.067265
3501.737148	328230.278152	43.072269
3501.608657	328195.654459	43.077274
3501.426501	328185.534007	43.082279
3501.553486	328169.158835	43.087284
3501.715488	328171.677145	43.092289
3501.398188	328151.988435	43.097293
3501.743228	328139.776104	43.102298
3501.913208	328127.209598	43.107303
3501.565075	328111.646326	43.112308
3501.501780	328088.738367	43.117313
3501.511332	328089.271066	43.122317
3501.487603	328084.874372	43.127322
3501.545438	328062.074640	43.132327
3501.407838	328048.284391	43.137332
3501.515911	328038.347453	43.142337
3501.730344	328041.493477	43.147341
3501.615012	328020.653937	43.152346
3501.680155	328010.265853	43.157351
3501.179899	328006.884785	43.162356
3501.493396	327988.013076	43.167361
3501.402593	327976.530174	43.172365
3501.793696	327959.375975	43.177370
3501.701270	327949.394052	43.182375
3501.206103	327939.322473	43.187380
3501.192270	327921.239554	43.192385
3501.544898	327924.363983	43.197389
3501.632322	327913.005816	43.202394
3501.631712	327902.475366	43.207399
3501.661487	327893.949623	43.212404
3501.590139	327874.069705	43.217409
3501.395977	327872.268689	43.222413
3501.473876	327867.754337	43.227418
3501.318244	327840.333024	43.232423
3501.442138	327839.728657	43.237428
3501.718463	327823.711539	43.242433
3501.427094	327830.624910	43.247437
3501.695218	327812.701351	43.252442
3501.492061	327793.147235	43.257447
3501.205521	327786.044478	43.262452
3501.744734	327782.170211	43.267457
3501.352548	327777.118871	43.272461
3501.158096	327760.208749	43.277466
3501.745659	327752.918459	43.282471
3501.541052	327745.853758	43.287476
3501.649596	327738.460300	43.292481
3501.764963	327721.781524	43.297485
3501.512145	327698.674043	43.302490
3501.760629	327700.848190	43.307495
3501.466787	327685.683244	43.312500
3501.755787	327665.238159	43.317505
3501.406215	327664.758683	43.322509
3501.293559	327658.620737	43.327514
3501.442534	327639.240420	43.332519
3501.588205	327633.443628	43.337524
3501.517301	327624.882695	43.342529
3501.104855	327619.376647	43.347533
3501.570465	327614.496416	43.352538
3501.388851	327585.858044	43.357543
3501.344545	327575.537830	43.362548
3501.810002	327561.373331	43.367553
3501.543740	327568.638932	43.372557
3501.448362	327541.894776	43.377562
3501.475712	327536.472578	43.382567
3501.473838	327539.805078	43.387572
3501.251737	327534.599934	43.392577
3501.609934	327519.612787	43.397581
3501.750668	327491.432680	43.402586
3501.678669	327491.164171	43.407591
3501.339876	327476.972758	43.412596
3501.527816	327457.255587	43.417601
3501.449564	327448.568582	43.422605
3501.388521	327440.336741	43.427610
3501.459908	327442.742082	43.432615
3501.477320	327433.658571	43.437620
3501.503363	327402.952683	43.442625
3501.586175	327399.073423	43.447629
3501.305752	327401.533767	43.452634
3501.343316	327394.863565	43.457639
3501.173596	327371.208734	43.462644
3501.759502	327366.360540	43.467649
3501.647952	327367.598968	43.472653
3501.632104	327358.775005	43.477658
3501.844623	327329.133678	43.482663
3501.372376	327333.379139	43.487668
3501.614040	327323.039589	43.492673
3501.431013	327303.329465	43.497677
3501.397639	327278.991913	43.502682
3501.384386	327274.568054	43.507687
3501.309393	327285.517546	43.512692
3501.311752	327273.409398	43.517697
3501.213885	327287.389419	43.522701
3501.208579	327250.507226	43.527706
3501.242456	327245.109405	43.532711
3501.131155	327238.004590	43.537716
3501.306826	327231.490825	43.542721
3501.357535	327231.660990	43.547725
3501.265588	327241.646552	43.552730
3501.178319	327219.606685	43.557735
3501.171178	327210.806764	43.562740
3501.658597	327205.897638	43.567745
3501.547155	327211.282225	43.572749
3501.357707	327201.798578	43.577754
3501.556092	327187.345024	43.582759
3501.577825	327178.337089	43.587764
3501.757940	327157.705275	43.592769
3501.765341	327168.641917	43.597773
3501.574688	327143.260531	43.602778
3501.425635	327128.835837	43.607783
3501.222265	327116.683495	43.612788
3501.387086	327112.689639	43.617793
3501.704095	327119.050160	43.622797
3501.313249	327093.013250	43.627802
3501.694074	327077.233862	43.632807
3501.349400	327086.139759	43.637812
3501.321233	327065.336965	43.642817
3501.307729	327052.697060	43.647821
3501.383506	327049.810898	43.652826
3501.239168	327040.778022	43.657831
3501.185788	327050.350615	43.662836
3501.294198	327031.892068	43.667841
3501.272747	327026.426557	43.672845
3501.630653	327015.509146	43.677850
3501.744567	326994.760413	43.682855
3501.224790	326999.038776	43.687860
3501.245324	326991.557192	43.692865
3501.515082	326981.696461	43.697869
3501.318437	326964.811781	43.702874
3501.557953	326956.151300	43.707879
3501.108619	326959.909918	43.712884
3501.461348	326953.241243	43.717889
3501.348475	326934.461131	43.722893
3501.439380	326924.857278	43.727898
3501.402876	326922.471960	43.732903
3501.401662	326911.407171	43.737908
3501.398136	326911.941931	43.742913
3501.654500	326890.509517	43.747917
3501.766118	326872.610005	43.752922
3501.581044	326860.480161	43.757927
3501.412607	326865.644774	43.762932
3501.518732	326836.935443	43.767937
3501.612013	326834.784198	43.772941
3501.488010	326828.673335	43.777946
3501.543024	326818.490020	43.782951
3501.486066	326799.472171	43.787956
3501.651937	326795.122003	43.792961
3501.855643	326780.489412	43.797965
3501.582821	326769.492483	43.802970
3501.785075	326744.685342	43.807975
3501.402380	326749.425601	43.812980
3501.339569	326735.139904	43.817985
3501.626934	326725.810532	43.822989
3501.417294	326710.504867	43.827994
3501.054408	326705.270750	43.832999
3500.956878	326710.729541	43.838004
3501.188673	326698.330980	43.843009
3501.103992	326704.245628	43.848013
3501.543273	326685.760630	43.853018
3501.978941	326677.120297	43.858023
3501.591166	326668.481513	43.863028
3501.741600	326654.900121	43.868033
3501.748403	326638.263304	43.873037
3501.569951	326633.814327	43.878042
3501.360059	326616.397395	43.883047
3501.221631	326606.880194	43.888052
3501.519656	326589.307531	43.893057
3501.445302	326590.260361	43.898061
3501.834398	326577.989793	43.903066
3501.827144	326582.493317	43.908071
3501.493871	326563.365933	43.913076
3501.384473	326554.200299	43.918081
3501.711854	326547.662706	43.923085
3501.678531	326532.812711	43.928090
3501.703729	326505.540271	43.933095
3501.261753	326512.019547	43.938100
3501.326473	326495.500801	43.943105
3501.193434	326483.922325	43.948109
3501.531483	326464.766251	43.953114
3501.467055	326465.921029	43.958119
3501.374035	326467.589019	43.963124
3501.396759	326462.701579	43.968129
3501.112712	326443.642753	43.973133
3501.483400	326435.928263	43.978138
3501.492865	326424.429239	43.983143
3501.356145	326431.547607	43.988148
3501.715865	326416.127380	43.993153
3501.423599	326400.427520	43.998157
3500.968048	326388.721376	44.003162
3501.577402	326386.667486	44.008167
3501.399699	326373.747792	44.013172
3501.305507	326361.196594	44.018177
3501.289209	326358.502838	44.023181
3501.168107	326340.486850	44.028186
3501.327365	326343.260077	44.033191
3501.451195	326342.782884	44.038196
3501.843900	326322.422651	44.043201
3501.437641	326315.007666	44.048205
3501.493295	326298.312196	44.053210
3501.561969	326301.786393	44.058215
3501.458962	326297.274710	44.063220
3501.594551	326281.126355	44.068225
3501.407963	326268.538699	44.073229
3501.265835	326254.214357	44.078234
3501.277954	326242.638554	44.083239
3501.329554	326250.617816	44.088244
3501.939824	326227.552612	44.093249
3501.699143	326212.429670	44.098253
3501.263177	326218.221247	44.103258
3501.672095	326209.025377	44.108263
3501.856796	326190.554517	44.113268
3501.722569	326167.402173	44.118273
3501.738842	326168.442594	44.123277
3501.422151	326137.077076	44.128282
3501.634457	326121.806970	44.133287
3501.155649	326129.589368	44.138292
3501.612471	326114.382781	44.143297
3501.357558	326102.441688	44.148301
3501.166054	326088.353943	44.153306
3501.572110	326088.366808	44.158311
3501.014602	326083.544597	44.163316
3501.374996	326066.775952	44.168321
3501.522077	326064.260133	44.173325
3501.198326	326053.118345	44.178330
3501.330641	326048.747906	44.183335
3501.001866	326047.654660	44.188340
3501.199875	326032.208694	44.193345
3501.476277	326032.597952	44.198349
3501.340202	326027.964222	44.203354
3501.416541	326005.643737	44.208359
3501.267242	326003.047063	44.213364
3501.304944	325989.126948	44.218369
3501.410491	325992.086658	44.223373
3501.399102	325991.783226	44.228378
3501.525450	325976.679127	44.233383
3501.157057	325972.870270	44.238388
3501.170918	325957.809188	44.243393
3501.450427	325958.961085	44.248397
3501.166417	325959.005522	44.253402
3501.456732	325959.468919	44.258407
3501.178342	325931.709368	44.263412
3501.439979	325920.654088	44.268417
3501.472291	325918.385139	44.273421
3501.184097	325917.209233	44.278426
3501.012003	325927.945337	44.283431
3501.131482	325923.093580	44.288436
3501.466175	325908.033196	44.293441
3501.283879	325891.222134	44.298445
3501.299240	325888.854084	44.303450
3501.427693	325886.977103	44.308455
3501.414220	325878.635755	44.313460
3501.540527	325872.332989	44.318465
3501.266284	325855.459974	44.323469
3501.707877	325841.069665	44.328474
3501.822852	325832.148602	44.333479
3501.404568	325825.244156	44.338484
3501.558068	325805.531560	44.343489
3501.349091	325801.977577	44.348493
3501.395932	325796.806473	44.353498
3501.716352	325787.624343	44.358503
3501.417309	325763.683534	44.363508
3501.158053	325771.762365	44.368513
3501.268550	325771.796000	44.373517
3501.024468	325755.630480	44.378522
3501.257380	325762.792929	44.383527
3501.198732	325750.642986	44.388532
3501.158973	325739.075149	44.393537
3501.022257	325721.773578	44.398541
3500.891009	325724.922954	44.403546
3501.402964	325712.785542	44.408551
3501.076854	325714.210191	44.413556
3501.216265	325711.339423	44.418561
3501.037233	325718.515406	44.423565
3501.204875	325701.903933	44.428570
3501.557718	325704.596064	44.433575
3501.337436	325692.267873	44.438580
3501.441227	325669.968349	44.443585
3501.556586	325676.843939	44.448589
3501.407128	325666.717738	44.453594
3501.560315	325651.990887	44.458599
3501.224458	325637.162423	44.463604
3501.491138	325636.942703	44.468609
3501.342222	325627.477786	44.473613
3501.296705	325628.298942	44.478618
3501.550831	325614.828178	44.483623
3501.406675	325596.713712	44.488628
3501.300939	325586.326279	44.493633
3501.584488	325594.218533	44.498637
3501.335368	325588.127041	44.503642
3501.855830	325558.105580	44.508647
3501.355946	325553.986550	44.513652
3501.851219	325544.700717	44.518657
3501.467576	325526.928913	44.523661
3501.679309	325509.318398	44.528666
3501.929510	325501.953259	44.533671
3501.103830	325493.815124	44.538676
3501.778280	325466.186103	44.543681
3501.651766	325466.841861	44.548685
3501.517498	325462.080595	44.553690
3501.582882	325451.208496	44.558695
3501.455724	325438.331475	44.563700
3501.355659	325428.807999	44.568705
3501.213157	325426.566353	44.573709
3501.514987	325417.946677	44.578714
3501.430167	325398.856211	44.583719
3501.274342	325386.645038	44.588724
3501.502874	325382.513863	44.593729
3501.417412	325382.145693	44.598733
3501.181448	325379.384463	44.603738
3501.300928	325358.837523	44.608743
3501.058840	325347.402958	44.613748
3501.189724	325328.456801	44.618753
3501.349309	325339.293833	44.623757
3501.306959	325343.370539	44.628762
3501.614955	325331.137712	44.633767
3501.297489	325330.093554	44.638772
3501.440103	325310.356983	44.643777
3501.417487	325301.991508	44.648781
3501.140192	325300.813880	44.653786
3501.118981	325293.999892	44.658791
3501.158081	325302.566365	44.663796
3501.547056	325295.764563	44.668801
3501.416136	325272.102434	44.673805
3501.308759	325261.511672	44.678810
3501.761379	325253.835026	44.683815
3501.577698	325262.461774	44.688820
3501.521271	325241.509832	44.693825
3501.589459	325229.390780	44.698829
3500.941261	325230.713172	44.703834
3501.284024	325220.433593	44.708839
3500.981674	325228.392078	44.713844
3501.358240	325225.484200	44.718849
3501.501859	325203.737827	44.723853
3501.151489	325189.165848	44.728858
3501.355274	325175.244927	44.733863
3501.158402	325181.482591	44.738868
3501.157233	325178.175881	44.743873
3501.344897	325172.957244	44.748877
3501.185714	325161.357039	44.753882
3501.464291	325138.215884	44.758887
3501.120264	325144.959881	44.763892
3500.861532	325126.710490	44.768897
3501.070377	325143.644979	44.773901
3501.006724	325133.657858	44.778906
3501.223093	325133.802133	44.783911
3501.211498	325130.420735	44.788916
3501.241542	325128.330163	44.793921
3501.204010	325115.795159	44.798925
3501.214787	325095.570337	44.803930
3501.354635	325092.699457	44.808935
3501.560074	325088.546424	44.813940
3501.424371	325090.144830	44.818945
3501.146225	325094.156672	44.823949
3501.113032	325076.431634	44.828954
3501.154797	325058.745746	44.833959
3501.373710	325066.877149	44.838964
3501.153450	325053.632992	44.843969
3501.325519	325047.348382	44.848973
3501.030710	325046.326112	44.853978
3501.317227	325056.125855	44.858983
3501.228069	325051.815372	44.863988
3501.323678	325016.238138	44.868993
3501.439867	325012.735001	44.873997
3501.049814	325007.784728	44.879002
3501.433043	325013.346652	44.884007
3500.973687	325017.971906	44.889012
3500.907771	325012.513075	44.894017
3501.221801	325005.646628	44.899021
3501.320441	324984.059798	44.904026
3501.099775	324975.114707	44.909031
3501.130519	324971.624925	44.914036
3501.260298	324967.967032	44.919041
3501.474820	324964.830088	44.924045
3501.261726	324960.793352	44.929050
3501.288902	324956.591861	44.934055
3501.388978	324947.825562	44.939060
3501.238779	324928.719659	44.944065
3501.064849	324929.179334	44.949069
3501.054606	324923.966168	44.954074
3501.550619	324914.069562	44.959079
3501.283632	324925.405841	44.964084
3501.737999	324905.518583	44.969089
3501.607365	324892.616496	44.974093
3501.126172	324890.351456	44.979098
3501.068818	324884.331631	44.984103
3501.071874	324889.138988	44.989108
3501.374044	324892.042601	44.994113
3501.561961	324869.754926	44.999117
3501.180310	324859.334129	45.004122
3501.374416	324839.487528	45.009127
3501.414514	324844.314537	45.014132
3501.627005	324830.417577	45.019137
3501.421095	324820.732439	45.024141
3501.124944	324811.061407	45.029146
3501.861962	324802.144622	45.034151
3501.600882	324796.436453	45.039156
3501.448072	324781.680813	45.044161
3501.573538	324773.571899	45.049165
3501.287385	324772.675460	45.054170
3501.566075	324765.000476	45.059175
3501.384570	324753.581712	45.064180
3501.433404	324730.476245	45.069185
3501.479926	324725.941009	45.074189
3501.459252	324728.513534	45.079194
3501.254792	324715.928191	45.084199
3501.467617	324702.234640	45.089204
3501.445086	324689.341026	45.094209
3501.365380	324688.793883	45.099213
3501.393226	324688.484306	45.104218
3501.421863	324668.281918	45.109223
3501.061858	324661.647982	45.114228
3501.300181	324646.653077	45.119233
3501.647772	324657.231953	45.124237
3501.195875	324641.708998	45.129242
3501.501143	324646.265630	45.134247
3501.285265	324632.104876	45.139252
3500.985591	324610.300300	45.144257
3501.364323	324597.827252	45.149261
3501.489532	324598.952435	45.154266
3501.157685	324602.260449	45.159271
3501.459710	324597.608940	45.164276
3501.370694	324580.808192	45.169281
3501.250774	324572.635849	45.174285
3501.236954	324573.706453	45.179290
3501.793664	324569.701958	45.184295
3501.238164	324573.070378	45.189300
3501.535708	324547.738233	45.194305
3501.516258	324535.658115	45.199309
3501.127336	324534.548792	45.204314
3501.717607	324519.218995	45.209319
3501.286494	324519.668005	45.214324
3501.040578	324506.300491	45.219329
3501.300993	324491.581897	45.224333
3501.205689	324492.588927	45.229338
3501.306721	324485.399556	45.234343
3500.940773	324493.266373	45.239348
3501.006383	324481.071187	45.244353
3501.172313	324485.318923	45.249357
3501.093428	324484.873401	45.254362
3500.869050	324486.841830	45.259367
3500.890051	324487.143842	45.264372
3501.137515	324481.763138	45.269377
3501.211813	324461.782455	45.274381
3501.070479	324450.230134	45.279386
3501.370427	324439.270218	45.284391
3500.985289	324448.030386	45.289396
3501.276183	324442.973586	45.294401
3501.097035	324446.893699	45.299405
3501.296191	324445.717873	45.304410
3501.586818	324431.605055	45.309415
3501.120194	324423.741269	45.314420
3501.390758	324410.521923	45.319425
3501.421841	324405.480298	45.324429
3501.297941	324408.755818	45.329434
3501.258067	324403.521779	45.334439
3500.927297	324381.136861	45.339444
3501.180944	324363.392109	45.344449
3501.213522	324366.694045	45.349453
3500.903747	324361.603950	45.354458
3501.470505	324356.682081	45.359463
3501.363689	324371.122397	45.364468
3501.213081	324371.145979	45.369473
3501.126295	324360.348256	45.374477
3501.187901	324347.441381	45.379482
3501.064959	324333.978270	45.384487
3500.962398	324338.166243	45.389492
3500.797687	324328.907001	45.394497
3501.120671	324332.901253	45.399501
3501.083863	324331.126353	45.404506
3501.178269	324324.980966	45.409511
3501.247234	324327.870201	45.414516
3501.176024	324326.024364	45.419521
3501.078952	324330.567617	45.424525
3501.103918	324322.067312	45.429530
3501.011642	324317.019524	45.434535
3501.143425	324301.506941	45.439540
3501.342324	324284.279483	45.444545
3501.269182	324280.195361	45.449549
3500.943185	324287.496325	45.454554
3501.374502	324284.935960	45.459559
3501.362447	324285.090511	45.464564
3501.377102	324282.391778	45.469569
3501.118170	324265.413958	45.474573
3501.029547	324250.444584	45.479578
3501.441278	324239.975909	45.484583
3501.150182	324243.735474	45.489588
3501.300475	324240.023431	45.494593
3500.974932	324238.573491	45.499597
3501.045269	324244.820399	45.504602
3501.370711	324231.694170	45.509607
3501.394609	324215.740530	45.514612
3501.089633	324192.333935	45.519617
3501.117974	324197.137420	45.524621
3500.988315	324203.212093	45.529626
3501.156846	324194.409493	45.534631
3501.333244	324193.415287	45.539636
3501.068361	324204.904067	45.544641
3500.560574	324195.672992	45.549645
3500.508768	324201.226724	45.554650
3501.465691	324191.893851	45.559655
3501.180769	324181.559512	45.564660
3501.492795	324176.957270	45.569665
3501.398560	324175.827304	45.574669
3501.207381	324159.347619	45.579674
3501.378025	324149.806960	45.584679
3501.253649	324146.188729	45.589684
3501.409340	324155.220546	45.594689
3501.240084	324144.588292	45.599693
3501.206679	324118.569905	45.604698
3501.111358	324105.662049	45.609703
3501.296208	324108.685815	45.614708
3501.343982	324115.597672	45.619713
3501.319306	324111.353325	45.624717
3501.164324	324107.917944	45.629722
3501.305336	324075.690689	45.634727
3500.969185	324089.352922	45.639732
3501.153742	324079.886389	45.644737
3501.269625	324076.993747	45.649741
3500.876315	324084.661410	45.654746
3501.210062	324080.208393	45.659751
3501.169826	324077.441912	45.664756
3501.248592	324081.652440	45.669761
3501.443793	324072.693012	45.674765
3501.205564	324057.899589	45.679770
3501.063426	324047.085000	45.684775
3500.793404	324046.186022	45.689780
3501.286717	324025.122074	45.694785
3501.013580	324037.426227	45.699789
3500.863496	324037.271656	45.704794
3501.103247	324033.367539	45.709799
3500.819807	324034.022414	45.714804
3501.008979	324031.016557	45.719809
3500.994442	324029.161846	45.724813
3501.099601	324034.640183	45.729818
3500.977349	324030.258450	45.734823
3501.110512	324010.242906	45.739828
3501.132630	323959.489380	45.744833
3501.015338	323858.007357	45.749837
3500.898041	323719.918652	45.754842
3500.878638	323520.302885	45.759847
3500.458659	323283.149840	45.764852
3500.185520	322988.581555	45.769857
3500.309228	322657.926888	45.774861
3499.937351	322288.831423	45.779866
3499.829587	321853.573053	45.784871
3499.335810	321388.274765	45.789876
3499.170632	320848.150287	45.794881
3498.394077	320277.127560	45.799885
3497.813163	319663.554334	45.804890
3497.771572	318988.726393	45.809895
3497.171869	318278.483578	45.814900
3496.456426	317512.909937	45.819905
3496.316281	316698.687930	45.824909
3495.319517	315846.292598	45.829914
3494.781025	314929.970601	45.834919
3494.003096	313979.928181	45.839924
3493.057647	312985.719736	45.844929
3492.679947	311934.403115	45.849933
3491.673485	310843.439800	45.854938
3490.842515	309705.754649	45.859943
3489.639083	308513.618011	45.864948
3488.628234	307266.734374	45.869953
3487.992005	305981.969567	45.874957
3486.260145	304669.934413	45.879962
3485.862948	303289.832720	45.884967
3484.757236	301876.235853	45.889972
3483.227235	300421.232881	45.894977
3482.238644	298906.828276	45.899981
3480.607838	297355.397907	45.904986
3479.635421	295765.998116	45.909991
3478.513516	294132.160390	45.914996
3477.375640	292441.388270	45.920001
3475.811407	290716.016020	45.925005
3474.218236	288953.561497	45.930010
3473.179794	287129.416500	45.935015
3471.226530	285294.060818	45.940020
3469.736445	283390.965396	45.945025
3468.328364	281469.474947	45.950029
3466.756028	279497.396035	45.955034
3464.906486	277488.849290	45.960039
3462.980718	275452.408292	45.965044
3461.031491	273366.218476	45.970049
3459.597344	271245.267896	45.975053
3457.531613	269098.520373	45.980058
3455.994918	266896.053512	45.985063
3453.735165	264686.061869	45.990068
3451.593628	262411.425973	45.995073
3449.717709	260121.575069	46.000077
3447.588666	257811.677390	46.005082
3445.392674	255430.977011	46.010087
3443.710726	253050.612730	46.015092
3441.035403	250621.366550	46.020097
3438.876964	248163.250126	46.025101
3436.268615	245674.379568	46.030106
3434.204480	243161.198224	46.035111
3431.152513	240622.191330	46.040116
3428.878742	238064.064352	46.045121
3426.457482	235464.680463	46.050125
3423.512799	232847.482255	46.055130
3421.095872	230201.357790	46.060135
3418.137208	227540.104394	46.065140
3415.495180	224854.780064	46.070145
3412.798499	222125.556221	46.075149
3410.108990	219401.303245	46.080154
3407.646841	216641.547098	46.085159
3404.343137	213857.412080	46.090164
3401.480921	211058.228558	46.095169
3398.343749	208230.641640	46.100173
3394.658779	205390.694234	46.105178
3391.799159	202531.963664	46.110183
3388.169639	199669.527705	46.115188
3385.179111	196785.498218	46.120193
3381.957229	193888.727753	46.125197
3378.303775	190982.463014	46.130202
3375.042899	188063.042215	46.135207
3371.513046	185146.949282	46.140212
3367.649579	182213.676686	46.145217
3364.297963	179271.680818	46.150221
3360.126435	176323.544903	46.155226
3356.319991	173364.074826	46.160231
3352.091023	170426.855398	46.165236
3348.172380	167486.762524	46.170241
3343.444207	164545.238028	46.175245
3338.766669	161620.355250	46.180250
3334.696927	158685.481117	46.185255
3330.007254	155777.672666	46.190260
3325.192314	152867.329447	46.195265
3320.338937	149978.483226	46.200269
3315.068877	147121.388473	46.205274
3309.761535	144280.920889	46.210279
3303.799634	141470.043458	46.215284
3298.060296	138626.353740	46.220289
3292.200012	135899.643335	46.225293
3285.238695	133206.763080	46.230298
3278.341307	130568.594902	46.235303
3270.872019	127994.480167	46.240308
3263.822772	125475.861809	46.245313
3256.280356	123018.879469	46.250317
3248.330247	120656.374273	46.255322
3240.095524	118361.620806	46.260327
3231.584071	116154.598324	46.265332
3222.949750	114040.966520	46.270337
3214.506621	112014.012917	46.275341
3205.315876	110080.241537	46.280346
3196.218369	108248.966217	46.285351
3186.876537	106519.144665	46.290356
3177.958046	104901.603570	46.295361
3168.830193	103380.830027	46.300365
3159.311317	101981.740805	46.305370
3150.651870	100678.730358	46.310375
3142.312274	99465.847675	46.315380
3133.906060	98352.129141	46.320385
3126.719899	97315.707392	46.325389
3118.860368	96371.308296	46.330394
3111.710430	95508.858639	46.335399
3104.822826	94715.485028	46.340404
3098.575558	93983.155487	46.345409
3092.454122	93307.460530	46.350413
3086.321292	92715.814643	46.355418
3080.630567	92157.898801	46.360423
3075.607098	91645.150170	46.365428
3070.609076	91163.511786	46.370433
3066.424502	90731.079870	46.375437
3061.880526	90321.035099	46.380442
3057.799573	89920.008307	46.385447
3053.889677	89546.620750	46.390452
3049.889573	89190.315711	46.395457
3046.729699	88847.669055	46.400461
3042.818851	88524.443302	46.405466
3039.559153	88212.973269	46.410471
3036.057946	87897.681915	46.415476
3032.615314	87591.443442	46.420481
3029.481791	87292.287252	46.425485
3025.905280	86996.659075	46.430490
3022.903457	86697.767849	46.435495
3019.770244	86403.511954	46.440500
3016.502591	86107.831750	46.445505
3013.173502	85816.013538	46.450509
3009.696776	85519.622452	46.455514
3006.775142	85212.120527	46.460519
3002.853309	84922.843158	46.465524
2999.338918	84635.194566	46.470529
2996.277170	84346.537990	46.475533
2993.072817	84050.208306	46.480538
2989.786993	83756.092098	46.485543
2986.172016	83462.297152	46.490548
2982.426969	83181.012697	46.495553
2979.072124	82881.847746	46.500557
2975.512359	82597.974075	46.505562
2972.256806	82303.868102	46.510567
2968.547894	82029.931543	46.515572
2965.091238	81741.007407	46.520577
2961.446903	81459.000232	46.525581
2957.801393	81187.297542	46.530586
2954.446253	80905.187178	46.535591
2950.445945	80631.462212	46.540596
2946.870433	80362.703409	46.545601
2943.855299	80085.844782	46.550605
2939.837073	79815.344141	46.555610
2936.562961	79544.729756	46.560615
2932.162741	79291.059873	46.565620
2928.744357	79031.993160	46.570625
2925.469517	78766.670184	46.575629
2921.621074	78519.728866	46.580634
2918.221244	78256.932426	46.585639
2914.759278	78009.020780	46.590644
2911.107465	77750.726544	46.595649
2907.061001	77513.655514	46.600653
2903.362095	77272.480752	46.605658
2900.056787	77024.591607	46.610663
2896.474953	76786.755699	46.615668
2892.940237	76549.524102	46.620673
2889.611766	76311.805118	46.625677
2885.709465	76074.000161	46.630682
2882.558737	75835.546357	46.635687
2879.062040	75600.958649	46.640692
2875.272933	75361.338901	46.645697
2872.218545	75130.368963	46.650701
2868.666975	74896.405530	46.655706
2865.048720	74649.971265	46.660711
2861.616619	74416.247310	46.665716
2858.307689	74172.613641	46.670721
2854.726035	73938.485478	46.675725
2851.215922	73707.357776	46.680730
2848.364808	73459.773187	46.685735
2844.783109	73221.740143	46.690740
2841.256227	72977.580033	46.695745
2837.957456	72736.878514	46.700749
2834.093016	72493.080413	46.705754
2831.006576	72246.661364	46.710759
2827.188543	71999.787625	46.715764
2823.537176	71768.927457	46.720769
2819.958745	71514.808431	46.725773
2816.196753	71276.135415	46.730778
2813.153967	71036.768002	46.735783
2809.652578	70790.490961	46.740788
2805.974795	70553.157273	46.745793
2802.613391	70305.974093	46.750797
2799.691903	70066.748943	46.755802
2795.954302	69819.997418	46.760807
2792.336443	69573.616757	46.765812
2788.663800	69329.234023	46.770817
2785.468289	69088.689491	46.775821
2781.990052	68834.409483	46.780826
2778.795323	68583.826682	46.785831
2775.283365	68350.321457	46.790836
2771.618107	68090.917038	46.795841
2768.129539	67843.878793	46.800845
2764.610489	67599.742329	46.805850
2761.245665	67346.874847	46.810855
2758.075188	67097.077173	46.815860
2754.429645	66842.284428	46.820865
2750.799954	66587.180712	46.825869
2747.237588	66333.890774	46.830874
2743.581629	66077.742574	46.835879
2740.119069	65828.282308	46.840884
2736.500299	65578.766412	46.845889
2733.129920	65320.581764	46.850893
2729.587821	65070.792298	46.855898
2725.928090	64819.354391	46.860903
2722.524109	64580.973131	46.865908
2719.341182	64323.429472	46.870913
2715.719724	64071.351999	46.875917
2711.944570	63825.527453	46.880922
2708.983522	63563.869454	46.885927
2705.386062	63307.575241	46.890932
2701.851492	63054.986673	46.895937
2698.785674	62793.073878	46.900941
2694.877533	62545.600868	46.905946
2691.526727	62280.913796	46.910951
2687.839450	62016.497956	46.915956
2684.537459	61763.797287	46.920961
2681.020634	61505.097417	46.925965
2677.652640	61257.889150	46.930970
2674.155502	60980.019567	46.935975
2670.443596	60730.776132	46.940980
2667.000960	60471.751859	46.945985
2663.344023	60208.315280	46.950989
2659.747108	59949.955256	46.955994
2656.276327	59686.831509	46.960999
2653.122968	59426.935392	46.966004
2649.568294	59179.066561	46.971009
2646.156923	58906.835785	46.976013
2642.420242	58655.662931	46.981018
2639.292252	58387.124880	46.986023
2635.646727	58117.928336	46.991028
2632.111417	57865.361559	46.996033
2629.023199	57600.918806	47.001037
2625.123275	57331.466248	47.006042
2621.578066	57068.693484	47.011047
2618.005458	56799.665234	47.016052
2614.839145	56533.476142	47.021057
2611.402852	56261.938995	47.026061
2607.476695	56008.754925	47.031066
2604.418833	55733.827158	47.036071
2600.667272	55472.747512	47.041076
2597.116211	55199.984140	47.046081
2593.894497	54933.758114	47.051085
2590.500639	54673.519549	47.056090
2586.785429	54393.621765	47.061095
2583.276597	54123.662094	47.066100
2579.916750	53857.799688	47.071105
2576.109426	53588.127578	47.076109
2572.451249	53325.274281	47.081114
2568.977706	53055.518006	47.086119
2565.809493	52786.878034	47.091124
2561.918822	52516.990194	47.096129
2558.731585	52250.186426	47.101133
2554.796912	51979.220530	47.106138
2551.824246	51715.104481	47.111143
2548.066495	51442.347245	47.116148
2544.456930	51181.324764	47.121153
2541.003344	50912.966706	47.126157
2537.419693	50648.952011	47.131162
2534.125610	50369.347352	47.136167
2530.764605	50104.422317	47.141172
2527.256196	49842.961430	47.146177
2523.996868	49573.554599	47.151181
2520.325683	49293.520870	47.156186
2517.134300	49007.719466	47.161191
2513.335633	48734.398060	47.166196
2509.987143	48468.132551	47.171201
2506.442212	48187.204602	47.176205
2502.732394	47912.230011	47.181210
2499.332055	47638.567656	47.186215
2495.705831	47361.024222	47.191220
2492.167294	47090.802388	47.196225
2489.172726	46818.164675	47.201229
2485.603006	46542.461729	47.206234
2482.573631	46255.083966	47.211239
2478.432312	45977.200469	47.216244
2474.776548	45691.855898	47.221249
2471.905538	45403.741224	47.226253
2468.133206	45135.412237	47.231258
2464.647940	44854.586129	47.236263
2461.081371	44571.296626	47.241268
2457.893637	44293.119944	47.246273
2454.536764	44010.806739	47.251277
2450.801600	43734.701250	47.256282
2447.351479	43440.126295	47.261287
2443.650576	43151.694889	47.266292
2440.234272	42880.344233	47.271297
2437.051960	42588.528875	47.276301
2433.114337	42306.588198	47.281306
2430.082334	42013.945254	47.286311
2426.988576	41709.217283	47.291316
2422.967383	41428.353526	47.296321
2419.374615	41133.508277	47.301325
2415.965894	40844.363871	47.306330
2412.441777	40558.988654	47.311335
2408.965932	40259.552609	47.316340
2405.215295	39976.667895	47.321345
2402.341291	39681.412776	47.326349
2398.467392	39402.137131	47.331354
2395.029045	39101.018300	47.336359
2391.490662	38819.351794	47.341364
2387.902554	38519.367661	47.346369
2384.660407	38222.364070	47.351373
2381.084006	37932.156140	47.356378
2377.697809	37631.797730	47.361383
2374.485024	37341.851526	47.366388
2370.999237	37046.309691	47.371393
2367.450604	36741.367574	47.376397
2363.709064	36434.932178	47.381402
2360.266181	36141.938233	47.386407
2356.796455	35842.080761	47.391412
2353.263212	35543.708134	47.396417
2349.966752	35245.543536	47.401421
2346.348040	34947.186319	47.406426
2343.358742	34635.961960	47.411431
2339.470291	34327.874756	47.416436
2336.145057	34036.159232	47.421441
2332.689156	33724.672662	47.426445
2328.671866	33416.872471	47.431450
2325.744071	33107.974594	47.436455
2322.265848	32801.639325	47.441460
2318.744128	32487.100968	47.446465
2315.238485	32182.997427	47.451469
2311.618269	31879.835259	47.456474
2308.638468	31560.219009	47.461479
2305.087009	31245.862461	47.466484
2301.683007	30931.760123	47.471489
2298.386821	30610.097497	47.476493
2294.909340	30294.159375	47.481498
2291.305760	29963.244986	47.486503
2288.133714	29649.252570	47.491508
2284.355645	29318.838446	47.496513
2281.167828	28985.498228	47.501517
2277.714828	28671.032368	47.506522
2274.190051	28335.632497	47.511527
2270.934507	28020.258556	47.516532
2267.248240	27677.144741	47.521537
2263.945516	27342.011588	47.526541
2259.977396	27015.364994	47.531546
2256.948679	26674.332304	47.536551
2253.501685	26351.315352	47.541556
2249.665129	26013.182818	47.546561
2246.598014	25679.972799	47.551565
2242.706160	25343.564545	47.556570
2239.680921	25000.018773	47.561575
2236.091607	24660.387619	47.566580
2232.327387	24319.896235	47.571585
2229.005359	23974.329976	47.576589
2225.223590	23637.597282	47.581594
2222.117598	23298.040311	47.586599
2218.159325	22962.936795	47.591604
2214.896628	22621.756012	47.596609
2211.454149	22286.880937	47.601613
2207.777000	21946.422771	47.606618
2204.508035	21600.376257	47.611623
2200.938297	21264.904877	47.616628
2197.206744	20921.938953	47.621633
2194.140233	20578.374519	47.626637
2190.516487	20232.230135	47.631642
2186.542014	19890.118338	47.636647
2182.679719	19555.893712	47.641652
2178.714396	19227.410604	47.646657
2174.941397	18916.669786	47.651661
2170.776730	18609.212819	47.656666
2166.896989	18296.218392	47.661671
2162.988515	18000.581497	47.666676
2158.793163	17706.514056	47.671681
2155.209740	17412.222332	47.676685
2151.448369	17144.506276	47.681690
2147.464200	16858.446294	47.686695
2143.646269	16592.890567	47.691700
2139.531388	16328.746589	47.696705
2135.745482	16073.037913	47.701709
2131.705586	15827.210676	47.706714
2128.020047	15585.773683	47.711719
2123.984999	15356.968255	47.716724
2120.101102	15129.889755	47.721729
2116.568704	14902.043364	47.726733
2112.706685	14678.677759	47.731738
2109.006594	14463.154447	47.736743
2105.782944	14256.190182	47.741748
2101.999780	14049.958450	47.746753
2098.375842	13840.503048	47.751757
2094.667760	13636.736831	47.756762
2091.181163	13425.960069	47.761767
2088.299506	13228.046529	47.766772
2084.667737	13014.846520	47.771777
2081.318477	12812.780671	47.776781
2077.480556	12607.504007	47.781786
2074.666955	12404.139821	47.786791
2071.410419	12203.047425	47.791796
2067.983058	11997.083154	47.796801
2064.463031	11785.734741	47.801805
2061.002772	11583.493655	47.806810
2057.781345	11373.214350	47.811815
2054.333374	11159.180317	47.816820
2050.406588	10950.510336	47.821825
2047.008104	10737.280627	47.826829
2043.261450	10532.094664	47.831834
2039.940092	10315.866188	47.836839
2036.459737	10106.648274	47.841844
2032.903719	9908.261078	47.846849
2030.013552	9693.593083	47.851853
2025.918437	9488.099604	47.856858
2022.480093	9279.720079	47.861863
2019.027434	9068.075310	47.866868
2015.436221	8869.318531	47.871873
2012.842841	8649.098985	47.876877
2008.967964	8452.464329	47.881882
2005.593581	8237.018488	47.886887
2001.756245	8023.553040	47.891892
1998.048856	7812.494230	47.896897
1994.874025	7601.924224	47.901901
1991.299852	7395.919850	47.906906
1987.739489	7177.565626	47.911911
1984.269637	6971.242673	47.916916
1980.797816	6767.248597	47.921921
1977.606315	6552.942712	47.926925
1973.742307	6349.356463	47.931930
1970.538551	6130.810134	47.936935
1966.806311	5924.777374	47.941940
1963.422741	5712.714090	47.946945
1960.253345	5497.151184	47.951949
1956.805068	5295.356669	47.956954
1953.123627	5077.340744	47.961959
1949.444182	4871.039457	47.966964
1945.749312	4660.261840	47.971969
1942.459169	4449.331563	47.976973
1938.832919	4251.642946	47.981978
1935.473375	4025.791845	47.986983
1931.573761	3823.707717	47.991988
1928.096004	3621.335159	47.996993
1924.636956	3405.449993	48.001997
1920.671814	3203.392545	48.007002
1917.219141	2997.504287	48.012007
1913.707395	2799.617435	48.017012
1910.201980	2596.975901	48.022017
1907.404977	2408.452095	48.027021
1903.126137	2200.161369	48.032026
1899.707330	1991.149948	48.037031
1896.143881	1803.467520	48.042036
1892.199164	1598.020330	48.047041
1888.854885	1395.984125	48.052045
1885.142918	1210.428908	48.057050
1881.380247	1014.445616	48.062055
1877.493076	827.222746	48.067060
1874.122579	652.181115	48.072065
1870.094921	466.505856	48.077069
1866.495745	297.736322	48.082074
1862.638092	143.711080	48.087079
1856.585113	33.314546	48.092084
1846.274934	61.010356	48.097089
1839.371540	54.345722	48.102093
1834.612664	70.327334	48.107098
1831.519167	56.786348	48.112103
1828.732081	64.606845	48.117108
1826.055351	77.415210	48.122113
1823.805418	68.731524	48.127117
1821.009499	74.541232	48.132122
1818.430889	68.515956	48.137127
1814.896805	54.930030	48.142132
1810.744524	71.155249	48.147137
1807.726755	58.140268	48.152141
1804.141005	74.779878	48.157146
1800.291857	74.657770	48.162151
1797.346987	70.002794	48.167156
1794.071436	65.579907	48.172161
1790.876207	62.675731	48.177165
1787.362362	68.755985	48.182170
1784.023855	65.671750	48.187175
1780.804052	69.443874	48.192180
1776.822647	68.513557	48.197185
1773.510149	68.630183	48.202189
1770.129754	70.260241	48.207194
1766.535925	63.735790	48.212199
1763.333191	55.087342	48.217204
1759.843233	70.930509	48.222209
1756.657566	65.946231	48.227213
1753.060211	67.806403	48.232218
1749.455310	69.762671	48.237223
1745.937468	59.315884	48.242228
1742.561507	66.371167	48.247233
1738.984991	67.225159	48.252237
1735.444680	73.559511	48.257242
1732.329536	67.827039	48.262247
1728.827398	66.302873	48.267252
1725.193325	72.148858	48.272257
1722.164977	68.098602	48.277261
1718.436317	69.381377	48.282266
1714.745088	70.670951	48.287271
1711.727253	67.071476	48.292276
1707.925421	71.222615	48.297281
1704.333496	62.622441	48.302285
1700.844513	67.271957	48.307290
1697.490367	72.340140	48.312295
1694.095825	60.687653	48.317300
1690.275656	75.383439	48.322305
1686.931130	55.940189	48.327309
1683.659576	58.252437	48.332314
1680.120799	70.322525	48.337319
1677.082057	68.517043	48.342324
1672.908849	72.944618	48.347329
1669.759408	69.454340	48.352333
1666.146440	71.446700	48.357338
1662.920197	71.037327	48.362343
1659.314472	67.852585	48.367348
1655.793166	66.113143	48.372353
1652.922184	57.292591	48.377357
1648.818181	71.985349	48.382362
1645.091655	59.989367	48.387367
1641.933191	62.008679	48.392372
1638.042606	62.706212	48.397377
1634.900061	60.309541	48.402381
1631.147351	64.481491	48.407386
1627.662065	72.847910	48.412391
1624.730116	64.976553	48.417396
1620.889539	67.349405	48.422401
1617.580665	68.243807	48.427405
1613.736873	68.677758	48.432410
1610.345051	63.849186	48.437415
1606.902211	64.451344	48.442420
1603.340056	65.464487	48.447425
1599.844117	55.492070	48.452429
1596.351792	56.114631	48.457434
1593.046602	72.017499	48.462439
1589.321742	53.532346	48.467444
1585.782807	64.406565	48.472449
1582.593605	60.217016	48.477453
1579.020344	62.266465	48.482458
1575.852154	61.591767	48.487463
1572.292001	63.993512	48.492468
1568.448769	67.160910	48.497473
1565.068371	57.815836	48.502477
1561.534971	61.909190	48.507482
1558.051712	63.400388	48.512487
1554.364026	62.920903	48.517492
1550.796503	61.384887	48.522497
1547.445160	55.806515	48.527501
1543.862177	68.165131	48.532506
1540.612391	65.589120	48.537511
1537.310044	64.647527	48.542516
1533.133453	65.108288	48.547521
1530.067475	65.578717	48.552525
1526.475987	73.974442	48.557530
1523.063767	58.876263	48.562535
1519.315799	70.596314	48.567540
1516.013116	70.581772	48.572545
1512.674219	58.082251	48.577549
1509.227630	63.848333	48.582554
1505.865509	58.315956	48.587559
1502.288538	63.555112	48.592564
1498.240560	63.261757	48.597569
1495.397270	63.020290	48.602573
1491.480355	62.380553	48.607578
1488.069252	67.796235	48.612583
1484.460731	69.439943	48.617588
1481.144238	74.869295	48.622593
1477.761606	65.110147	48.627597
1474.321835	62.731578	48.632602
1470.370077	59.664349	48.637607
1466.811832	66.232541	48.642612
1463.640100	61.872618	48.647617
1460.168286	64.513676	48.652621
1456.794558	65.687203	48.657626
1452.787537	57.765888	48.662631
1449.820652	56.173859	48.667636
1446.055260	63.574920	48.672641
1443.198589	67.388376	48.677645
1439.013052	63.699684	48.682650
1435.378882	54.527268	48.687655
1431.910214	55.288553	48.692660
1428.218171	61.599285	48.697665
1425.303940	55.930391	48.702669
1421.752557	64.145855	48.707674
1417.654338	57.096219	48.712679
1414.357097	67.170178	48.717684
1410.889555	61.217734	48.722689
1408.034508	63.199112	48.727693
1404.621226	61.091672	48.732698
1400.826861	53.915387	48.737703
1397.350781	53.855259	48.742708
1393.298984	62.342052	48.747713
1389.891669	56.990802	48.752717
1386.385706	68.331317	48.757722
1382.907980	64.291406	48.762727
1379.884032	58.532133	48.767732
1376.058793	65.721119	48.772737
1373.035234	57.661714	48.777741
1369.226617	62.484751	48.782746
1365.294937	56.544870	48.787751
1361.975416	57.238538	48.792756
1358.887381	59.095047	48.797761
1355.300250	52.284980	48.802765
1351.296414	63.551575	48.807770
1347.896963	58.110524	48.812775
1344.718704	60.161496	48.817780
1341.170911	57.107017	48.822785
1337.538377	50.746996	48.827789
1334.207890	61.345036	48.832794
1330.695146	60.999602	48.837799
1327.206025	57.511997	48.842804
1323.677399	71.924948	48.847809
1320.279079	56.524133	48.852813
1316.441167	54.654042	48.857818
1313.076256	59.771474	48.862823
1309.637242	54.975717	48.867828
1305.513636	59.677240	48.872833
1302.538185	62.699396	48.877837
1299.382590	51.882888	48.882842
1295.544899	52.085049	48.887847
1292.493011	54.369357	48.892852
1288.640143	53.716511	48.897857
1285.064743	57.832345	48.902861
1281.369069	65.092829	48.907866
1278.138647	59.318457	48.912871
1274.364069	62.127195	48.917876
1270.749602	59.959549	48.922881
1267.723115	40.207310	48.927885
1264.261247	52.056640	48.932890
1260.687444	55.561622	48.937895
1257.220882	57.641934	48.942900
1253.349161	63.711929	48.947905
1250.113819	51.430439	48.952909
1246.414163	67.069252	48.957914
1242.905611	61.382727	48.962919
1239.656260	46.423714	48.967924
1235.641218	60.957119	48.972929
1232.178268	57.965331	48.977933
1229.023163	61.294045	48.982938
1225.649399	60.300463	48.987943
1222.387353	51.031923	48.992948
1218.369293	60.219016	48.997953
1215.125498	49.590360	49.002957
1211.564445	56.051498	49.007962
1208.105872	47.715410	49.012967
1204.753977	53.669237	49.017972
1200.808678	56.359194	49.022977
1197.217856	56.073489	49.027981
1193.795988	64.015640	49.032986
1190.238602	66.046918	49.037991
1187.169558	57.561267	49.042996
1183.618389	55.579900	49.048001
1180.088342	58.445303	49.053005
1176.442865	59.626664	49.058010
1172.765991	62.986460	49.063015
1169.598248	60.704623	49.068020
1165.905823	58.362559	49.073025
1162.869394	61.213965	49.078029
1159.237984	63.320119	49.083034
1155.219667	68.210863	49.088039
1152.060798	58.641455	49.093044
1148.432768	62.132819	49.098049
1144.932337	56.106539	49.103053
1141.650890	61.976592	49.108058
1137.992807	61.331276	49.113063
1134.709497	63.398759	49.118068
1131.006159	62.624488	49.123073
1127.674016	60.928393	49.128077
1123.945832	54.539144	49.133082
1120.148696	62.138268	49.138087
1116.952731	52.486100	49.143092
1113.541930	46.616648	49.148097
1110.285910	47.882594	49.153101
1106.693806	47.356676	49.158106
1102.602399	49.778477	49.163111
1099.744473	45.967514	49.168116
1095.866679	52.997135	49.173121
1092.263944	50.131692	49.178125
1088.945640	55.634202	49.183130
1085.479296	53.275758	49.188135
1082.212557	51.477691	49.193140
1078.282265	55.655484	49.198145
1074.848446	55.797664	49.203149
1071.455314	49.181975	49.208154
1067.817383	58.588014	49.213159
1064.529687	48.466174	49.218164
1060.771383	53.420645	49.223169
1057.155212	48.975432	49.228173
1054.042788	52.946088	49.233178
1050.381799	56.135759	49.238183
1047.299249	52.670030	49.243188
1043.044342	52.542141	49.248193
1039.640372	44.137467	49.253197
1036.487344	42.024219	49.258202
1032.767367	47.153033	49.263207
1029.565924	53.826843	49.268212
1025.632228	59.555440	49.273217
1022.672698	54.922007	49.278221
1019.037529	48.518243	49.283226
1015.045820	46.700831	49.288231
1012.430189	48.992846	49.293236
1008.210394	54.598563	49.298241
1004.940101	50.804738	49.303245
1001.438728	42.203359	49.308250
997.870136	57.097200	49.313255
994.275227	57.169717	49.318260
990.506976	60.116775	49.323265
987.849436	43.559263	49.328269
983.861807	58.499737	49.333274
979.922226	52.830191	49.338279
977.147937	54.837007	49.343284
972.989116	46.297450	49.348289
969.745908	48.453619	49.353293
966.609489	54.066893	49.358298
962.976056	55.698867	49.363303
959.369733	49.727213	49.368308
955.752460	55.456910	49.373313
952.118783	51.517521	49.378317
948.468238	60.359257	49.383322
945.232794	59.404230	49.388327
942.061958	47.688586	49.393332
938.354869	54.220131	49.398337
934.807922	37.542481	49.403341
931.395899	51.946745	49.408346
927.742907	49.658717	49.413351
924.433984	50.025004	49.418356
921.064999	51.862361	49.423361
917.355379	47.884258	49.428365
914.052662	47.803486	49.433370
910.446076	52.303980	49.438375
906.969482	49.096156	49.443380
903.104285	50.444901	49.448385
899.602759	49.597994	49.453389
896.049510	46.478108	49.458394
892.856100	41.894001	49.463399
889.256545	46.867966	49.468404
885.438375	53.802902	49.473409
882.324790	49.956112	49.478413
878.823966	55.749859	49.483418
875.496741	53.047007	49.488423
872.005460	50.749498	49.493428
868.013147	62.476352	49.498433
864.619938	46.698478	49.503437
861.459355	58.130576	49.508442
857.362482	49.685781	49.513447
854.118389	52.645725	49.518452
850.608820	54.982848	49.523457
847.945280	51.157348	49.528461
844.011969	52.735083	49.533466
840.353585	48.094090	49.538471
836.733746	49.081737	49.543476
833.052271	51.964643	49.548481
829.468207	55.003142	49.553485
826.106808	48.325638	49.558490
822.506605	49.699359	49.563495
819.083350	54.715346	49.568500
815.941729	56.118500	49.573505
812.208862	48.588006	49.578509
808.707560	53.720621	49.583514
805.177377	52.878237	49.588519
801.763658	42.428235	49.593524
797.862914	45.854856	49.598529
794.702586	45.138058	49.603533
791.504209	51.169209	49.608538
787.751417	43.126154	49.613543
784.543315	39.161325	49.618548
780.391677	51.406697	49.623553
777.031855	49.474620	49.628557
773.386374	44.932877	49.633562
770.054037	58.141456	49.638567
767.087689	45.292878	49.643572
762.974916	49.119714	49.648577
760.025771	44.858075	49.653581
756.414404	49.463775	49.658586
752.387538	54.542670	49.663591
749.176696	43.232015	49.668596
745.472020	54.711378	49.673601
742.133529	43.116993	49.678605
738.567049	48.455991	49.683610
735.333635	45.121569	49.688615
732.085945	46.155381	49.693620
728.132794	45.154637	49.698625
724.605814	45.292551	49.703629
720.914683	51.236373	49.708634
717.348814	58.910145	49.713639
713.520552	55.678375	49.718644
710.434729	46.629232	49.723649
707.217943	39.116048	49.728653
703.592339	49.194145	49.733658
699.982890	53.530645	49.738663
696.736029	52.995112	49.743668
693.172123	40.208512	49.748673
689.788720	43.706017	49.753677
686.551833	47.411534	49.758682
682.644628	52.832386	49.763687
679.130268	39.671037	49.768692
675.253456	46.058406	49.773697
672.221978	37.177944	49.778701
668.873260	49.810139	49.783706
664.682111	35.913229	49.788711
661.688836	42.488100	49.793716
658.092738	39.276947	49.798721
654.693004	35.813580	49.803725
650.979199	43.953462	49.808730
647.579344	43.128695	49.813735
644.087126	33.776236	49.818740
640.142388	41.607437	49.823745
637.048424	40.399409	49.828749
633.485467	43.349249	49.833754
629.898107	40.449952	49.838759
626.786928	42.199577	49.843764
622.779124	43.874491	49.848769
619.573745	38.969661	49.853773
615.921577	35.150375	49.858778
612.125314	41.680174	49.863783
609.353420	39.947150	49.868788
605.515816	48.214006	49.873793
602.375974	46.839168	49.878797
598.497057	40.910369	49.883802
594.599335	43.963273	49.888807
591.843556	36.055233	49.893812
587.902114	37.672312	49.898817
584.469728	48.460504	49.903821
580.620180	49.152030	49.908826
577.155817	43.819540	49.913831
574.167956	45.451793	49.918836
570.232689	51.965416	49.923841
567.107682	45.890080	49.928845
563.281928	47.998416	49.933850
560.055030	40.828562	49.938855
556.423685	47.832428	49.943860
552.713200	45.097979	49.948865
549.517207	41.321169	49.953869
546.265076	46.414846	49.958874
542.520123	49.867788	49.963879
539.092095	31.191215	49.968884
535.310599	47.877561	49.973889
531.786210	33.857318	49.978893
528.465344	42.375460	49.983898
525.050644	38.120386	49.988903
521.587707	52.086633	49.993908
517.834771	43.246463	49.998913
514.014737	47.432513	50.003917
511.111085	56.701571	50.008922
507.474846	52.977909	50.013927
504.038470	45.144859	50.018932
500.036386	50.915999	50.023937
496.940700	46.408487	50.028941
493.728492	42.532997	50.033946
489.679391	51.734693	50.038951
486.374320	35.886269	50.043956
482.919080	45.485331	50.048961
479.249787	40.653219	50.053965
475.884404	42.097860	50.058970
472.323814	40.801625	50.063975
468.722717	33.282299	50.068980
465.093262	51.270467	50.073985
461.950973	48.345820	50.078989
458.685863	38.948381	50.083994
454.690987	45.256247	50.088999
451.580710	47.113356	50.094004
447.974540	54.369583	50.099009
444.251630	50.982228	50.104013
440.976270	55.810659	50.109018
437.239418	43.228446	50.114023
434.194966	37.618276	50.119028
430.406500	42.890909	50.124033
426.764117	45.878576	50.129037
423.244295	49.397542	50.134042
419.637306	48.178198	50.139047
416.048441	41.533338	50.144052
412.825007	54.835677	50.149057
409.525122	40.454460	50.154061
405.792165	36.312561	50.159066
402.089563	43.707291	50.164071
398.891114	39.902450	50.169076
395.216341	46.618944	50.174081
391.722442	45.780531	50.179085
388.675248	47.937829	50.184090
384.573223	54.907915	50.189095
381.245867	51.370044	50.194100
377.535661	45.940107	50.199105
374.274949	45.599850	50.204109
370.857307	47.479822	50.209114
367.188666	53.075398	50.214119
364.359367	39.221605	50.219124
360.579418	54.851069	50.224129
356.818340	49.188663	50.229133
353.039277	46.819384	50.234138
349.562037	46.788300	50.239143
346.370469	32.880535	50.244148
342.530566	47.911949	50.249153
339.372888	46.258426	50.254157
335.890627	41.741929	50.259162
332.163030	52.019618	50.264167
328.746726	46.698689	50.269172
324.845509	52.919171	50.274177
321.570720	38.742875	50.279181
318.216562	43.779840	50.284186
314.680500	46.599035	50.289191
311.214681	43.547956	50.294196
307.224923	54.034400	50.299201
304.151472	45.938945	50.304205
301.124240	45.448246	50.309210
297.515836	42.156916	50.314215
294.151149	45.920546	50.319220
290.157625	47.055528	50.324225
286.673789	38.666867	50.329229
283.242195	45.800886	50.334234
279.793704	49.106250	50.339239
276.324887	35.071106	50.344244
272.254923	47.000139	50.349249
268.963124	34.316666	50.354253
265.849514	40.420114	50.359258
261.879447	37.194948	50.364263
258.934990	36.302155	50.369268
255.031326	51.084159	50.374273
251.296420	50.783430	50.379277
248.179456	47.010175	50.384282
244.327149	39.486012	50.389287
241.082356	42.234296	50.394292
237.719114	43.998228	50.399297
234.559729	40.601784	50.404301
230.749384	45.321101	50.409306
227.149334	50.029623	50.414311
223.774024	44.683335	50.419316
219.644247	48.959154	50.424321
216.698371	50.904483	50.429325
213.286879	47.544377	50.434330
209.569978	48.218444	50.439335
206.422983	48.404600	50.444340
202.294466	51.114172	50.449345
198.857354	47.198101	50.454349
195.749873	51.661790	50.459354
191.925037	51.739006	50.464359
188.495713	40.975364	50.469364
184.968274	45.223272	50.474369
181.493813	40.743586	50.479373
177.746065	42.824041	50.484378
174.555008	38.720739	50.489383
171.231788	39.918442	50.494388
167.807609	46.178143	50.499393
164.259955	42.747641	50.504397
160.548872	40.108373	50.509402
156.863059	47.079781	50.514407
153.506915	33.726239	50.519412
149.752941	46.346128	50.524417
146.553192	44.911239	50.529421
142.876358	49.460979	50.534426
139.853523	42.234024	50.539431
136.646564	41.189410	50.544436
132.601592	45.018545	50.549441
128.832462	40.765382	50.554445
124.967086	41.010330	50.559450
121.759818	55.866774	50.564455
118.675858	47.488306	50.569460
115.278969	61.033034	50.574465
111.666776	44.631799	50.579469
108.178835	52.619427	50.584474
104.236355	49.994289	50.589479
100.925115	38.446563	50.594484
97.596221	43.894094	50.599489
94.227933	30.548815	50.604493
90.168521	33.551328	50.609498
86.940212	49.227318	50.614503
83.494758	39.766555	50.619508
80.109111	46.210074	50.624513
76.266301	40.775746	50.629517
73.045158	42.159972	50.634522
69.110441	54.159642	50.639527
65.987112	55.307084	50.644532
62.488864	53.434940	50.649537
59.014230	53.944564	50.654541
55.983939	45.636808	50.659546
52.050362	56.269568	50.664551
48.576680	49.470789	50.669556
44.576669	55.121566	50.674561
41.409450	54.675037	50.679565
37.949619	45.191235	50.684570
34.422084	58.155341	50.689575
31.086530	45.175112	50.694580
27.165845	54.176531	50.699585
24.238685	55.856399	50.704589
20.659666	54.715098	50.709594
16.610647	53.321573	50.714599
13.269862	48.643845	50.719604
9.582056	54.973382	50.724609
6.235215	49.803061	50.729613
3.311522	48.616038	50.734618