Fri Mar 05 19:37:15 2021

Number of Points = 14581

Depth (nm)	Load (N)	Time (s)
-0.102420	92.533221	0.000000
-0.269456	85.332795	0.005005
-0.597108	65.081903	0.010010
-2.845551	21.248239	0.015014
-6.512600	2.963555	0.020019
-11.976176	2.442743	0.025024
-17.200630	2.331651	0.030029
-21.639342	3.870868	0.035034
-26.411886	7.350950	0.040038
-29.680399	2.436732	0.045043
-33.563500	3.283369	0.050048
-36.716449	4.701082	0.055053
-40.238008	8.934101	0.060058
-44.061738	-2.073145	0.065062
-48.008062	-2.151527	0.070067
-52.004101	1.800812	0.075072
-55.590474	3.804932	0.080077
-58.849712	-1.755693	0.085082
-62.740033	-2.238798	0.090086
-66.671021	-1.305622	0.095091
-70.921561	9.619596	0.100096
-74.630203	2.985828	0.105101
-78.118045	-2.929380	0.110106
-82.082028	-1.828489	0.115110
-85.094091	4.685566	0.120115
-89.392717	4.354378	0.125120
-93.136857	9.168607	0.130125
-96.325755	4.363205	0.135130
-100.808609	7.789325	0.140134
-104.183657	-4.159878	0.145139
-108.244367	9.179374	0.150144
-111.873076	-3.672357	0.155149
-115.812622	3.800268	0.160154
-119.658777	2.963280	0.165158
-123.340336	-5.699522	0.170163
-127.022645	-0.754763	0.175168
-130.937530	-0.412252	0.180173
-134.861382	9.997322	0.185178
-138.757875	4.987920	0.190182
-142.309806	-4.714241	0.195187
-146.138672	3.895092	0.200192
-149.819073	0.746713	0.205197
-153.230359	-2.430410	0.210202
-157.225254	8.261767	0.215206
-160.717639	-3.493585	0.220211
-164.653282	7.641730	0.225216
-168.463370	6.007439	0.230221
-171.885011	4.472013	0.235226
-176.229171	9.669122	0.240230
-179.574090	0.526911	0.245235
-183.699601	-2.649728	0.250240
-187.404457	-2.865765	0.255245
-191.355713	1.115921	0.260250
-194.712791	-0.103348	0.265254
-198.308270	0.595149	0.270259
-202.480497	12.463713	0.275264
-206.153033	-0.234216	0.280269
-209.778758	1.222903	0.285274
-213.331735	9.526535	0.290278
-217.043508	-6.031988	0.295283
-220.982165	4.812157	0.300288
-224.962119	-5.278872	0.305293
-228.524730	-3.912223	0.310298
-232.760197	4.304822	0.315302
-236.168309	-2.909656	0.320307
-239.831444	4.790278	0.325312
-243.671828	5.575240	0.330317
-247.480602	7.851679	0.335322
-251.570805	10.980439	0.340326
-255.195700	-0.472921	0.345331
-259.090758	3.854715	0.350336
-262.412152	1.611142	0.355341
-265.817615	-1.076319	0.360346
-269.925271	5.980260	0.365350
-273.536618	4.289183	0.370355
-277.667977	14.408826	0.375360
-281.542896	10.135803	0.380365
-285.117853	5.452209	0.385370
-288.979829	7.732475	0.390374
-292.459026	7.097382	0.395379
-296.584920	4.911318	0.400384
-299.911331	4.318077	0.405389
-303.708734	7.808610	0.410394
-307.942209	10.501445	0.415398
-311.137750	7.599188	0.420403
-314.911480	10.146103	0.425408
-318.746534	8.618539	0.430413
-322.667627	3.578680	0.435418
-326.452925	10.624891	0.440422
-330.432514	2.338004	0.445427
-334.523307	5.331379	0.450432
-338.014525	9.973133	0.455437
-341.386305	9.617427	0.460442
-345.325897	6.576964	0.465446
-348.900842	6.955442	0.470451
-352.653464	13.581742	0.475456
-356.559319	5.425051	0.480461
-360.257242	6.955423	0.485466
-364.119927	7.493403	0.490470
-367.923420	4.571597	0.495475
-371.719281	3.774293	0.500480
-375.384192	6.330734	0.505485
-378.843676	1.406501	0.510490
-382.885187	8.216163	0.515494
-386.573815	5.388010	0.520499
-390.337890	6.408600	0.525504
-394.482736	-0.522427	0.530509
-397.768508	-2.410377	0.535514
-401.776592	5.021598	0.540518
-405.404341	1.699634	0.545523
-409.283151	5.326329	0.550528
-413.209197	5.734159	0.555533
-416.447106	4.538751	0.560538
-420.491181	5.922641	0.565542
-424.039869	2.788352	0.570547
-428.051382	8.025821	0.575552
-432.062206	3.803138	0.580557
-435.397575	8.450104	0.585562
-439.556893	7.173212	0.590566
-443.004485	-4.607768	0.595571
-446.865648	4.677371	0.600576
-450.856528	1.823472	0.605581
-454.303363	6.545033	0.610586
-458.231600	7.397983	0.615590
-461.766872	1.453084	0.620595
-466.016901	16.042099	0.625600
-469.452600	8.181097	0.630605
-472.861234	-3.702252	0.635610
-476.868982	10.373425	0.640614
-480.496473	3.664275	0.645619
-484.440509	6.308037	0.650624
-488.615623	5.528912	0.655629
-492.363191	8.076654	0.660634
-495.592179	17.204137	0.665638
-499.291193	4.208153	0.670643
-503.321224	9.057622	0.675648
-507.280547	15.028047	0.680653
-510.814619	1.903238	0.685658
-514.867092	10.594574	0.690662
-518.211211	7.129711	0.695667
-522.016752	7.936360	0.700672
-525.658926	0.816472	0.705677
-529.635265	-2.015961	0.710682
-533.468431	3.090690	0.715686
-537.184231	4.878075	0.720691
-540.802723	0.573990	0.725696
-544.648414	1.827052	0.730701
-548.495263	11.144755	0.735706
-552.355067	7.115773	0.740710
-555.700794	1.404090	0.745715
-559.506298	2.581372	0.750720
-563.436153	6.984434	0.755725
-567.186426	5.831657	0.760730
-571.080157	8.631525	0.765734
-574.602108	4.308916	0.770739
-578.584908	-1.203190	0.775744
-582.137939	6.280957	0.780749
-585.858759	0.589817	0.785754
-589.861661	6.420678	0.790758
-593.597182	0.020702	0.795763
-597.665308	1.952775	0.800768
-601.272164	7.103801	0.805773
-604.948779	0.300200	0.810778
-608.976685	0.727778	0.815782
-612.482147	7.332325	0.820787
-615.910909	-0.293017	0.825792
-619.894980	10.303534	0.830797
-623.500759	1.258859	0.835802
-627.577946	4.837172	0.840806
-631.275843	-2.946991	0.845811
-634.848355	5.557464	0.850816
-638.658575	12.470936	0.855821
-642.330243	-8.815951	0.860826
-646.275045	4.841496	0.865830
-650.066943	-0.779835	0.870835
-654.017760	3.945262	0.875840
-657.818677	6.200590	0.880845
-660.931899	10.473325	0.885850
-664.993625	7.120184	0.890854
-668.810720	1.256908	0.895859
-672.702099	1.412047	0.900864
-676.377244	4.027348	0.905869
-679.842095	-0.324722	0.910874
-683.786472	14.408190	0.915878
-687.590203	2.623001	0.920883
-691.581844	5.937019	0.925888
-695.299044	1.956452	0.930893
-698.530408	2.659014	0.935898
-702.839689	16.901497	0.940902
-706.587102	2.784517	0.945907
-709.858148	6.409183	0.950912
-713.666385	6.289332	0.955917
-717.596440	4.553676	0.960922
-721.710647	6.166898	0.965926
-725.489480	7.382760	0.970931
-729.139453	9.674002	0.975936
-733.059851	3.824189	0.980941
-736.298872	6.519691	0.985946
-739.893865	13.001534	0.990950
-743.668587	2.662584	0.995955
-747.638691	6.600872	1.000960
-751.623799	11.394687	1.005965
-755.546205	2.265214	1.010970
-759.426525	7.990028	1.015974
-762.809448	2.980023	1.020979
-766.373076	7.173493	1.025984
-770.441991	-2.344113	1.030989
-773.935441	2.457884	1.035994
-778.199209	7.901821	1.040998
-781.758494	-2.421031	1.046003
-785.689364	11.237560	1.051008
-789.242680	13.013557	1.056013
-792.544263	-2.552767	1.061018
-796.618586	5.951705	1.066022
-800.458724	9.022494	1.071027
-804.272551	15.282371	1.076032
-808.339118	8.918316	1.081037
-811.737544	8.509192	1.086042
-815.423402	10.047798	1.091046
-819.003013	2.675536	1.096051
-823.054607	-1.169369	1.101056
-827.013148	-3.712405	1.106061
-830.456701	-3.600208	1.111066
-834.536163	8.375971	1.116070
-837.945460	-2.689848	1.121075
-842.047924	-0.825987	1.126080
-845.288732	3.811148	1.131085
-849.023866	0.626893	1.136090
-852.985029	3.264535	1.141094
-856.931284	3.094441	1.146099
-860.536830	3.699350	1.151104
-864.608860	3.402723	1.156109
-868.288696	1.778704	1.161114
-871.974179	1.522791	1.166118
-875.688189	-0.658716	1.171123
-879.438239	0.499173	1.176128
-883.366820	1.717150	1.181133
-886.967449	-5.233752	1.186138
-890.871107	9.994422	1.191142
-893.975108	1.432927	1.196147
-897.972982	6.691061	1.201152
-901.988685	9.769583	1.206157
-905.780588	2.045056	1.211162
-909.730625	8.833067	1.216166
-913.425089	1.946092	1.221171
-917.295356	3.295148	1.226176
-921.230673	0.554597	1.231181
-924.485859	4.287402	1.236186
-928.381745	13.130986	1.241190
-931.885742	2.441571	1.246195
-936.065634	12.324044	1.251200
-940.138720	8.679896	1.256205
-943.275089	-1.661434	1.261210
-947.019917	0.687884	1.266214
-950.757099	0.184901	1.271219
-954.279773	11.376814	1.276224
-958.353136	6.581585	1.281229
-962.121783	-0.815409	1.286234
-965.909548	6.238474	1.291238
-969.581591	-6.470853	1.296243
-973.449889	-3.095669	1.301248
-977.437644	-0.861993	1.306253
-981.242975	0.456283	1.311258
-984.888416	8.058283	1.316262
-988.373220	-1.230641	1.321267
-992.242262	2.907926	1.326272
-995.931302	2.414662	1.331277
-999.300261	7.679614	1.336282
-1003.810049	10.600786	1.341286
-1007.467276	11.343494	1.346291
-1011.203947	9.063327	1.351296
-1014.871503	9.873930	1.356301
-1018.569651	9.490966	1.361306
-1022.549214	12.447218	1.366310
-1026.175671	10.187294	1.371315
-1030.021345	13.669339	1.376320
-1034.111782	13.932606	1.381325
-1037.289412	12.114991	1.386330
-1041.147735	7.140439	1.391334
-1044.887453	7.300321	1.396339
-1048.353299	-1.330807	1.401344
-1052.394606	6.090186	1.406349
-1056.272609	3.499969	1.411354
-1060.409065	18.513333	1.416358
-1063.827766	7.561330	1.421363
-1067.353251	-2.854770	1.426368
-1071.090174	6.458762	1.431373
-1075.093157	0.916062	1.436378
-1079.228028	5.890486	1.441382
-1082.613807	9.395241	1.446387
-1086.270319	2.686982	1.451392
-1090.075480	8.649454	1.456397
-1093.467720	-8.182348	1.461402
-1097.728418	7.421787	1.466406
-1101.447633	12.030142	1.471411
-1105.068950	10.264676	1.476416
-1109.095583	6.723784	1.481421
-1112.525986	-7.739648	1.486426
-1116.512063	-0.259579	1.491430
-1119.971272	2.336051	1.496435
-1124.125054	3.943688	1.501440
-1127.938121	13.816684	1.506445
-1131.053655	2.112982	1.511450
-1135.199591	13.155705	1.516454
-1138.684068	-3.853657	1.521459
-1142.770035	-0.202104	1.526464
-1147.051409	7.673763	1.531469
-1150.252601	6.716346	1.536474
-1154.055266	8.121206	1.541478
-1157.618357	7.152316	1.546483
-1161.226375	-5.011849	1.551488
-1165.171029	3.100328	1.556493
-1169.126049	-0.995953	1.561498
-1173.317441	3.828406	1.566502
-1176.665502	6.500951	1.571507
-1180.212650	-1.782651	1.576512
-1184.065198	-0.401299	1.581517
-1187.810605	-3.597547	1.586522
-1191.684970	10.423200	1.591526
-1195.671450	6.384036	1.596531
-1199.265132	4.674220	1.601536
-1203.189203	1.706854	1.606541
-1206.323568	-7.978407	1.611546
-1210.250252	12.885124	1.616550
-1214.076602	5.264405	1.621555
-1218.039647	4.641879	1.626560
-1222.084763	12.541574	1.631565
-1225.419383	4.123109	1.636570
-1229.494741	0.806268	1.641574
-1232.997984	3.946841	1.646579
-1236.721325	2.475449	1.651584
-1240.666476	11.224907	1.656589
-1244.401595	3.518680	1.661594
-1247.735834	7.624114	1.666598
-1251.711810	1.326792	1.671603
-1255.619625	-4.276544	1.676608
-1259.764196	13.285165	1.681613
-1262.863782	1.858220	1.686618
-1266.940681	16.129115	1.691622
-1270.402298	9.039888	1.696627
-1274.126326	2.949860	1.701632
-1278.301293	10.108776	1.706637
-1281.835398	-0.199941	1.711642
-1285.820712	12.936708	1.716646
-1289.313021	5.532310	1.721651
-1292.967036	5.275182	1.726656
-1297.181367	13.211547	1.731661
-1300.697143	5.224307	1.736666
-1304.205769	6.077734	1.741670
-1308.256335	0.768567	1.746675
-1311.670697	4.339722	1.751680
-1316.226543	13.250129	1.756685
-1319.459577	5.990355	1.761690
-1323.320927	12.473112	1.766694
-1326.899425	0.563114	1.771699
-1330.756210	1.694655	1.776704
-1334.658488	3.603023	1.781709
-1338.278626	-6.952017	1.786714
-1341.981030	2.369010	1.791718
-1345.923800	3.933802	1.796723
-1349.395738	-0.097569	1.801728
-1353.170093	0.396354	1.806733
-1357.003009	-9.023901	1.811738
-1360.718572	0.327644	1.816742
-1364.757980	-0.840634	1.821747
-1368.768139	2.661981	1.826752
-1372.462240	10.513616	1.831757
-1375.556770	-1.937390	1.836762
-1380.015117	7.880023	1.841766
-1383.617812	10.680357	1.846771
-1387.469312	-4.547825	1.851776
-1391.272531	3.598843	1.856781
-1394.798170	-4.982735	1.861786
-1398.652852	10.739825	1.866790
-1402.175506	4.046926	1.871795
-1405.336102	-8.410799	1.876800
-1409.587985	-3.748226	1.881805
-1413.174967	-6.403350	1.886810
-1417.280112	-2.969022	1.891814
-1421.209555	1.479526	1.896819
-1425.019746	7.099562	1.901824
-1428.714886	-1.705554	1.906829
-1432.527642	-6.484877	1.911834
-1436.114499	-3.459923	1.916838
-1440.157181	11.310381	1.921843
-1443.681830	5.745366	1.926848
-1447.424102	-3.958899	1.931853
-1450.863195	-1.094775	1.936858
-1455.113184	1.807737	1.941862
-1458.920486	4.606257	1.946867
-1462.302009	-6.147628	1.951872
-1466.220092	5.160348	1.956877
-1469.646279	5.092519	1.961882
-1473.689740	4.391850	1.966886
-1477.328273	-1.478140	1.971891
-1481.393665	-1.479862	1.976896
-1485.530367	12.923957	1.981901
-1488.794292	1.783854	1.986906
-1492.508202	4.767742	1.991910
-1496.025448	-1.255679	1.996915
-1500.253683	9.507695	2.006912
-1501.330830	3.847820	2.016909
-1498.620140	4.490778	2.026906
-1495.629929	9.975789	2.036902
-1493.503343	11.189133	2.046899
-1491.954029	6.141275	2.056896
-1489.763104	5.141700	2.066893
-1488.129742	10.701903	2.076890
-1486.059018	5.229501	2.086886
-1484.283914	7.204923	2.096883
-1482.211246	8.646384	2.106880
-1480.288868	5.994042	2.116877
-1478.426727	3.133455	2.126874
-1476.778768	6.324500	2.136870
-1474.950360	7.058243	2.146867
-1472.803974	5.650556	2.156864
-1470.661597	5.490873	2.166861
-1469.054074	5.423155	2.176858
-1467.109075	4.194562	2.186854
-1465.227398	2.538744	2.196851
-1463.489673	7.895939	2.206848
-1461.375820	7.257677	2.216845
-1459.155371	5.050252	2.226842
-1457.795530	2.120113	2.236838
-1456.010665	0.896645	2.246835
-1454.002103	1.309454	2.256832
-1452.105255	-2.286138	2.266829
-1450.083926	2.068817	2.276826
-1448.238487	6.879832	2.286822
-1446.221821	7.408192	2.296819
-1444.422974	5.999337	2.306816
-1442.842304	-0.480869	2.316813
-1440.702829	6.972003	2.326810
-1438.667900	12.970050	2.336806
-1436.993718	4.076463	2.346803
-1435.201362	4.156015	2.356800
-1433.119558	0.305034	2.366797
-1431.374439	1.235304	2.376794
-1429.268215	0.765661	2.386790
-1427.625415	2.984942	2.396787
-1425.899933	2.042582	2.406784
-1423.801049	0.623598	2.416781
-1421.845968	3.490775	2.426778
-1419.903697	0.175301	2.436774
-1418.219003	3.810505	2.446771
-1416.198953	1.159946	2.456768
-1414.546221	-1.643379	2.466765
-1412.639892	0.830560	2.476762
-1410.513890	-3.491684	2.486758
-1408.767291	-3.107946	2.496755
-1406.793749	-0.996867	2.506752
-1405.262441	-0.349711	2.516749
-1403.006157	-1.629667	2.526746
-1401.247858	-0.499379	2.536742
-1399.458171	0.731674	2.546739
-1397.357665	-6.141200	2.556736
-1395.473311	-5.391087	2.566733
-1393.875339	-5.408277	2.576730
-1391.676574	-3.489557	2.586726
-1390.311954	-1.566765	2.596723
-1388.243435	-3.707167	2.606720
-1386.142066	0.606612	2.616717
-1384.337199	-0.076849	2.626714
-1382.541356	3.182169	2.636710
-1380.299232	1.989765	2.646707
-1378.692947	6.764915	2.656704
-1376.732727	1.686085	2.666701
-1374.982756	2.554044	2.676698
-1373.204413	4.439036	2.686694
-1371.382281	7.188594	2.696691
-1369.104881	-1.960987	2.706688
-1367.153570	4.239983	2.716685
-1365.612000	5.944991	2.726682
-1363.981882	4.207947	2.736678
-1361.657703	4.998205	2.746675
-1359.838105	4.511351	2.756672
-1357.977857	4.769567	2.766669
-1356.147254	2.346753	2.776666
-1354.312728	2.571195	2.786662
-1352.514872	4.648869	2.796659
-1350.449529	4.593208	2.806656
-1348.421194	0.804543	2.816653
-1346.620656	-3.497125	2.826650
-1345.070799	0.691821	2.836646
-1343.090179	2.140249	2.846643
-1341.472572	3.916786	2.856640
-1339.320430	-2.768518	2.866637
-1337.457503	-1.227037	2.876634
-1335.191215	1.274612	2.886630
-1333.705870	3.241273	2.896627
-1331.709216	0.214006	2.906624
-1329.728410	-1.967569	2.916621
-1328.082639	0.156573	2.926618
-1325.845307	-0.864487	2.936614
-1324.229899	-3.972826	2.946611
-1322.273906	1.071650	2.956608
-1320.404437	-0.807886	2.966605
-1318.525307	-2.621072	2.976602
-1316.933007	1.319523	2.986598
-1315.152546	-1.210496	2.996595
-1312.864526	0.739804	3.006592
-1311.183683	-1.065322	3.016589
-1309.205901	-1.844296	3.026586
-1307.423005	5.542627	3.036582
-1305.364436	3.424415	3.046579
-1303.647313	6.680309	3.056576
-1301.657392	-2.536883	3.066573
-1299.627040	1.578347	3.076570
-1298.026208	1.507082	3.086566
-1296.091456	-2.200244	3.096563
-1294.152090	6.699535	3.106560
-1292.477799	2.977057	3.116557
-1290.782433	2.797508	3.126554
-1288.628847	-2.327990	3.136550
-1286.590660	2.453891	3.146547
-1284.756690	3.826367	3.156544
-1282.829438	2.011823	3.166541
-1281.078389	0.770215	3.176538
-1279.050559	0.652728	3.186534
-1277.382154	-1.183542	3.196531
-1275.458586	-2.136968	3.206528
-1273.857040	-6.493576	3.216525
-1271.304880	-7.596549	3.226522
-1269.838123	0.445735	3.236518
-1268.008171	-2.728483	3.246515
-1265.829658	1.412014	3.256512
-1264.304545	1.807625	3.266509
-1262.233956	-1.570889	3.276506
-1260.586303	0.254581	3.286502
-1258.855258	4.117752	3.296499
-1256.466329	2.633551	3.306496
-1254.752291	-1.879996	3.316493
-1252.493999	-0.913295	3.326490
-1251.058190	0.559245	3.336486
-1249.398622	-5.668205	3.346483
-1247.286309	-0.989731	3.356480
-1245.267845	-3.215156	3.366477
-1243.630572	-4.888525	3.376474
-1241.804789	-1.174713	3.386470
-1239.846828	1.597426	3.396467
-1238.026177	5.834694	3.406464
-1236.082980	-1.947608	3.416461
-1233.953314	-3.661873	3.426458
-1232.170032	2.300846	3.436454
-1230.402588	7.846105	3.446451
-1228.512525	2.491250	3.456448
-1226.542829	-3.646867	3.466445
-1224.858734	-2.532990	3.476442
-1222.933508	0.099139	3.486438
-1220.965459	1.477053	3.496435
-1219.014425	4.226634	3.506432
-1217.303546	8.931485	3.516429
-1215.501682	0.546553	3.526426
-1213.508704	2.237852	3.536422
-1211.679710	10.304323	3.546419
-1209.841096	6.280869	3.556416
-1207.493481	6.420166	3.566413
-1205.999984	5.639826	3.576410
-1204.464966	9.239146	3.586406
-1202.159254	11.868832	3.596403
-1200.132405	5.363166	3.606400
-1198.743009	4.673698	3.616397
-1196.545578	-0.924524	3.626394
-1194.595149	6.977267	3.636390
-1193.051463	7.436269	3.646387
-1191.114496	4.017617	3.656384
-1189.001919	6.097167	3.666381
-1187.213021	0.839058	3.676378
-1185.460309	-4.594836	3.686374
-1183.378797	-0.561896	3.696371
-1181.460293	0.975558	3.706368
-1179.641274	-2.054739	3.716365
-1178.138809	-1.249659	3.726362
-1175.871553	1.654626	3.736358
-1173.941674	4.477105	3.746355
-1172.191259	5.247254	3.756352
-1170.312411	-1.379968	3.766349
-1168.462971	-0.106189	3.776346
-1166.644335	0.171470	3.786342
-1165.005626	5.192644	3.796339
-1162.655135	4.674686	3.806336
-1160.883562	4.206724	3.816333
-1159.076970	-0.348408	3.826330
-1157.196315	7.706686	3.836326
-1155.282023	10.106941	3.846323
-1153.198285	2.951159	3.856320
-1151.494061	3.176084	3.866317
-1149.978268	5.090627	3.876314
-1147.624526	-3.603605	3.886310
-1146.090476	1.304853	3.896307
-1144.038020	-1.050662	3.906304
-1142.175433	1.681558	3.916301
-1140.484822	4.403399	3.926298
-1138.684140	-1.772347	3.936294
-1136.683149	0.612471	3.946291
-1134.538626	-0.292505	3.956288
-1132.750330	5.083708	3.966285
-1130.779611	2.082861	3.976282
-1129.026968	-5.743083	3.986278
-1127.187006	7.126430	3.996275
-1125.283511	4.542131	4.006272
-1123.454042	4.023882	4.016269
-1121.655439	2.585312	4.026266
-1119.612421	-2.009193	4.036262
-1117.793457	-2.396283	4.046259
-1116.050141	-1.940746	4.056256
-1113.874826	-1.246423	4.066253
-1112.135430	-0.889728	4.076250
-1110.351709	-1.568016	4.086246
-1108.461380	5.160839	4.096243
-1106.693984	1.145698	4.106240
-1104.669106	1.144098	4.116237
-1102.679345	-0.678722	4.126234
-1100.875290	3.529735	4.136230
-1098.890287	4.109255	4.146227
-1097.061354	-1.144142	4.156224
-1095.404589	-7.434201	4.166221
-1093.260029	-4.897049	4.176218
-1091.539237	2.038939	4.186214
-1089.726599	4.496562	4.196211
-1087.922751	3.175599	4.206208
-1085.973971	0.187772	4.216205
-1084.067621	7.670402	4.226202
-1081.876820	6.538596	4.236198
-1080.238689	9.191511	4.246195
-1078.452749	0.929219	4.256192
-1076.613292	4.655192	4.266189
-1074.462166	6.292895	4.276186
-1072.839878	1.263622	4.286182
-1070.621638	11.491108	4.296179
-1068.961875	-1.273093	4.306176
-1067.109860	-0.451222	4.316173
-1065.232515	1.209755	4.326170
-1063.592527	0.148705	4.336166
-1061.662779	-0.377641	4.346163
-1059.691034	2.848765	4.356160
-1057.638466	-1.248270	4.366157
-1055.750939	-3.784170	4.376154
-1054.164288	2.686990	4.386150
-1052.198921	-1.389777	4.396147
-1050.224355	0.230399	4.406144
-1048.273083	2.907459	4.416141
-1046.347752	2.077096	4.426138
-1044.431890	-1.505431	4.436134
-1042.701653	0.689093	4.446131
-1040.987170	-2.599116	4.456128
-1039.175033	-0.744530	4.466125
-1037.317301	0.640134	4.476122
-1035.353150	0.019886	4.486118
-1033.358770	1.404802	4.496115
-1031.173873	3.183986	4.506112
-1029.603476	-3.218536	4.516109
-1027.588903	-0.453688	4.526106
-1025.914757	1.345611	4.536102
-1024.155995	-1.333881	4.546099
-1022.015171	-1.123428	4.556096
-1020.179102	-2.054756	4.566093
-1018.076949	-1.939167	4.576090
-1016.586583	0.481636	4.586086
-1014.774719	-2.852130	4.596083
-1012.972335	2.094034	4.606080
-1010.822206	-1.712251	4.616077
-1008.688496	1.039876	4.626074
-1007.143049	-1.438119	4.636070
-1005.340342	-0.494628	4.646067
-1003.171618	4.464008	4.656064
-1001.417107	2.573106	4.666061
-999.587949	1.533951	4.676058
-997.795906	6.546520	4.686054
-995.832887	2.435435	4.696051
-993.710854	2.434183	4.706048
-991.839271	4.655089	4.716045
-990.160291	-0.162144	4.726042
-988.485253	3.476513	4.736038
-986.730314	4.915552	4.746035
-984.577515	5.079914	4.756032
-982.793823	7.138042	4.766029
-980.760534	1.035732	4.776026
-978.909539	6.559941	4.786022
-977.134382	4.517334	4.796019
-975.110486	-1.918204	4.806016
-973.273319	0.177168	4.816013
-971.574184	0.720406	4.826010
-969.476222	-2.635394	4.836006
-967.599619	-2.583165	4.846003
-965.637747	-3.034042	4.856000
-964.153242	0.614574	4.865997
-962.058916	-4.400111	4.875994
-960.309581	-4.951208	4.885990
-958.487130	1.382843	4.895987
-956.245580	0.129355	4.905984
-954.598114	-2.799130	4.915981
-952.678385	-0.364839	4.925978
-950.779396	4.126982	4.935974
-948.871502	-1.154724	4.945971
-946.994661	-1.006200	4.955968
-945.261107	0.605238	4.965965
-943.298603	-8.864665	4.975962
-941.064465	-3.389063	4.985958
-939.455845	3.812881	4.995955
-937.765319	3.370679	5.005952
-935.928690	-2.714358	5.015949
-934.035102	4.209919	5.025946
-932.076179	-3.252564	5.035942
-930.578719	-2.713364	5.045939
-928.206358	3.246994	5.055936
-926.252111	-4.350526	5.065933
-924.391008	-5.596836	5.075930
-922.630316	-0.517617	5.085926
-920.888550	1.406737	5.095923
-918.844017	0.585838	5.105920
-916.828469	-1.619897	5.115917
-915.020968	-2.342892	5.125914
-913.243471	-5.371088	5.135910
-911.148161	-4.493257	5.145907
-909.715741	-3.102065	5.155904
-907.828475	4.178509	5.165901
-905.918694	-1.772940	5.175898
-903.618681	1.716906	5.185894
-902.018979	-5.051802	5.195891
-900.161592	1.088818	5.205888
-898.421384	-3.973406	5.215885
-896.163128	2.919440	5.225882
-894.559448	-2.381479	5.235878
-892.722195	3.779736	5.245875
-890.705814	4.607048	5.255872
-888.934883	1.002023	5.265869
-886.906656	2.361129	5.275866
-884.886989	-0.424713	5.285862
-883.286696	2.070183	5.295859
-881.958700	2.762824	5.305856
-879.445659	7.813376	5.315853
-877.489918	-2.155929	5.325850
-875.712571	1.957508	5.335846
-873.757165	12.198804	5.345843
-871.709842	9.509602	5.355840
-870.170575	4.171625	5.365837
-868.343439	1.664472	5.375834
-866.305507	-1.380064	5.385830
-864.439424	0.949195	5.395827
-862.593896	-1.098262	5.405824
-860.890995	0.856035	5.415821
-858.685404	-4.654773	5.425818
-857.134553	-4.010377	5.435814
-855.111948	-1.958766	5.445811
-853.140612	-5.568960	5.455808
-851.262312	-5.520066	5.465805
-849.647087	-5.395957	5.475802
-847.665869	-0.550879	5.485798
-845.726734	1.875664	5.495795
-843.738416	0.959606	5.505792
-841.652195	8.734226	5.515789
-840.166420	2.814291	5.525786
-838.127656	8.993867	5.535782
-836.391754	5.588690	5.545779
-834.613730	7.080997	5.555776
-832.363727	-3.715316	5.565773
-830.571035	0.166756	5.575770
-829.447824	4.099010	5.585766
-826.890525	-1.161678	5.595763
-824.954333	0.065352	5.605760
-823.190489	-3.704282	5.615757
-821.362102	1.485777	5.625754
-819.362648	3.891649	5.635750
-817.588306	6.410875	5.645747
-815.718371	5.197974	5.655744
-813.743779	3.696766	5.665741
-811.827227	3.084313	5.675738
-810.350928	3.453288	5.685734
-808.182468	1.527937	5.695731
-806.151907	7.407274	5.705728
-804.492469	1.508548	5.715725
-802.960232	-0.555100	5.725722
-801.026100	1.881754	5.735718
-798.777588	-4.548495	5.745715
-796.639721	-0.311043	5.755712
-795.054516	3.391066	5.765709
-792.969881	-1.187719	5.775706
-791.208464	0.605697	5.785702
-789.555781	2.778074	5.795699
-787.538367	0.801096	5.805696
-785.616761	0.479961	5.815693
-783.857123	-2.238971	5.825690
-781.863921	1.926881	5.835686
-779.906863	-0.446234	5.845683
-778.264963	3.557878	5.855680
-776.535373	-0.111512	5.865677
-774.647782	1.042802	5.875674
-772.501317	-2.235319	5.885670
-770.399756	3.675333	5.895667
-768.669498	1.606898	5.905664
-766.954527	6.781974	5.915661
-765.091477	-0.072956	5.925658
-763.257899	-2.727902	5.935654
-761.191958	0.928974	5.945651
-759.486185	1.782359	5.955648
-757.499842	-3.952267	5.965645
-755.612994	6.112198	5.975642
-753.542575	1.941508	5.985638
-751.917044	-8.019138	5.995635
-750.106426	-0.151439	6.005632
-748.177612	2.947891	6.015629
-746.047618	-4.167583	6.025626
-744.403226	-4.515432	6.035622
-742.746064	-2.089526	6.045619
-740.838783	4.344837	6.055616
-738.715483	-3.492720	6.065613
-736.723340	-1.576663	6.075610
-735.293092	-3.785022	6.085606
-732.860510	4.752243	6.095603
-731.172626	2.587974	6.105600
-729.116116	-3.239949	6.115597
-727.477602	0.731582	6.125594
-725.470441	-0.206335	6.135590
-724.204620	-2.284200	6.145587
-722.012069	-4.156482	6.155584
-719.626497	-3.808024	6.165581
-718.151747	-3.184532	6.175578
-716.514058	-10.028671	6.185574
-714.647909	0.384925	6.195571
-712.409050	-8.795815	6.205568
-710.661890	-5.837953	6.215565
-708.523739	-8.423108	6.225562
-706.827748	-6.431278	6.235558
-705.205418	-5.749256	6.245555
-703.149283	0.662930	6.255552
-701.081596	-7.925183	6.265549
-699.154829	-4.302854	6.275546
-697.602139	-3.549698	6.285542
-695.998666	-1.134126	6.295539
-693.767754	0.983814	6.305536
-691.779097	-0.596910	6.315533
-689.758638	1.253084	6.325530
-688.043830	-0.337561	6.335526
-686.326605	-4.327017	6.345523
-684.293102	-1.238047	6.355520
-682.351302	-2.823907	6.365517
-680.636332	1.628075	6.375514
-678.688013	-2.385673	6.385510
-676.865520	0.091231	6.395507
-674.833616	-0.312176	6.405504
-673.368064	-0.945610	6.415501
-671.242547	0.576560	6.425498
-669.315448	-0.545887	6.435494
-667.592544	1.969043	6.445491
-665.548668	-1.616278	6.455488
-663.780169	-9.158657	6.465485
-661.598345	-3.060202	6.475482
-659.783369	1.344238	6.485478
-658.215427	-5.561355	6.495475
-656.393391	0.499858	6.505472
-654.262766	-4.070369	6.515469
-652.508615	-9.292547	6.525466
-650.477342	-3.252131	6.535462
-648.848912	1.535809	6.545459
-646.720879	-2.604523	6.555456
-645.105170	-6.721416	6.565453
-642.899351	-2.110990	6.575450
-641.322009	1.613010	6.585446
-639.408986	0.377573	6.595443
-637.626509	-2.011745	6.605440
-635.513356	-1.753887	6.615437
-633.356297	-2.864099	6.625434
-631.754126	0.266991	6.635430
-630.112310	-7.501443	6.645427
-628.061292	-0.136261	6.655424
-626.025412	-4.181325	6.665421
-624.134038	-5.444871	6.675418
-622.577919	0.068328	6.685414
-620.838638	4.505421	6.695411
-618.663259	-9.251956	6.705408
-616.865813	-4.407313	6.715405
-614.752509	-7.555261	6.725402
-613.042104	-4.664082	6.735398
-611.404599	0.597700	6.745395
-609.189695	-5.234905	6.755392
-607.309643	-3.717672	6.765389
-605.583900	-3.031577	6.775386
-603.593429	-1.636192	6.785382
-601.784427	-2.927613	6.795379
-600.091129	4.022640	6.805376
-597.853046	0.223189	6.815373
-596.140851	6.881480	6.825370
-594.476862	-0.629951	6.835366
-592.486315	3.364389	6.845363
-590.853212	0.940546	6.855360
-588.635698	-7.088782	6.865357
-586.642796	-8.985887	6.875354
-584.953233	-8.366629	6.885350
-583.053146	-4.725728	6.895347
-581.096899	-5.026968	6.905344
-579.315462	-4.635542	6.915341
-577.328335	-0.024851	6.925338
-575.414885	-1.715045	6.935334
-573.837046	0.035232	6.945331
-571.625810	-4.190960	6.955328
-569.707698	-1.757667	6.965325
-568.006651	-7.144990	6.975322
-566.030602	0.991703	6.985318
-564.604820	5.930501	6.995315
-562.515379	-0.339921	7.005312
-560.469927	2.322513	7.015309
-558.615104	-1.118836	7.025306
-556.741372	0.015763	7.035302
-555.113502	3.738069	7.045299
-552.701027	-7.461333	7.055296
-551.019055	2.866570	7.065293
-549.360406	3.085001	7.075290
-547.487953	2.670858	7.085286
-545.590404	1.149017	7.095283
-543.512488	1.736272	7.105280
-541.907679	0.084353	7.115277
-539.456699	-1.476937	7.125274
-538.017083	-3.538258	7.135270
-536.576431	0.232914	7.145267
-534.259889	-2.783219	7.155264
-532.127768	-5.373574	7.165261
-530.561158	-5.487798	7.175258
-528.638988	-3.372489	7.185254
-526.663637	-0.651460	7.195251
-525.005584	4.626054	7.205248
-523.133755	-1.691682	7.215245
-520.994724	-3.413128	7.225242
-519.155666	0.665473	7.235238
-517.641339	-1.142504	7.245235
-515.335982	-3.916831	7.255232
-513.297088	-3.724373	7.265229
-511.768980	-5.408231	7.275226
-510.277526	-8.088869	7.285222
-508.034544	2.687886	7.295219
-506.149643	-5.855093	7.305216
-504.419798	-10.591707	7.315213
-502.441350	-5.861144	7.325210
-500.238270	-4.512261	7.335206
-498.396622	-1.457220	7.345203
-496.888902	-1.500437	7.355200
-494.885408	-1.343361	7.365197
-492.805032	-4.493841	7.375194
-491.175415	-3.441781	7.385190
-489.211722	-4.336244	7.395187
-487.130995	-7.883092	7.405184
-485.350479	-6.618286	7.415181
-483.709688	-8.828547	7.425178
-481.912251	-4.844323	7.435174
-479.608552	-5.385709	7.445171
-478.074424	-10.678419	7.455168
-475.980643	-6.678361	7.465165
-474.075285	-8.624552	7.475162
-472.454350	-3.904760	7.485158
-470.565224	-2.088864	7.495155
-468.529015	-7.842282	7.505152
-466.563282	-3.935450	7.515149
-464.669048	-2.349313	7.525146
-462.867327	-8.152121	7.535142
-461.206782	-0.506527	7.545139
-459.111048	-7.668398	7.555136
-457.079427	-7.433677	7.565133
-455.774703	-6.703920	7.575130
-453.754147	-1.926353	7.585126
-451.709879	-3.506288	7.595123
-449.687277	-9.113832	7.605120
-447.920917	-6.544100	7.615117
-446.008870	-3.246047	7.625114
-444.177226	-3.562014	7.635110
-442.368788	-1.894263	7.645107
-440.511246	-5.695960	7.655104
-438.309639	-3.001513	7.665101
-436.725273	-6.176948	7.675098
-434.892826	-2.593016	7.685094
-432.844660	-7.173572	7.695091
-430.959355	-4.856506	7.705088
-429.348738	-5.841380	7.715085
-427.308238	-3.598040	7.725082
-425.550996	2.170553	7.735078
-423.572055	-1.885782	7.745075
-421.430644	2.627778	7.755072
-419.638825	-2.039730	7.765069
-417.793820	-1.126224	7.775066
-416.345120	-0.165224	7.785062
-414.237649	1.810064	7.795059
-412.137841	1.912356	7.805056
-410.378163	-9.237942	7.815053
-408.810046	-4.512828	7.825050
-406.444515	-2.046633	7.835046
-404.857526	-1.232444	7.845043
-402.844054	0.699442	7.855040
-401.074527	-5.497660	7.865037
-399.250302	0.222364	7.875034
-397.250435	-4.175189	7.885030
-395.436914	-3.078216	7.895027
-393.462496	-3.287467	7.905024
-391.609446	-7.854204	7.915021
-389.693386	2.910140	7.925018
-387.778731	6.000984	7.935014
-386.336539	3.784601	7.945011
-384.250919	0.213371	7.955008
-382.060956	1.054457	7.965005
-380.297658	-5.127426	7.975002
-378.473825	-2.069444	7.984998
-376.515514	2.816027	7.994995
-374.839417	-4.060881	8.004992
-373.154357	-8.483939	8.014989
-370.908089	-6.513406	8.024986
-369.248084	-1.210825	8.034982
-367.255171	-5.461979	8.044979
-365.074303	-5.183114	8.054976
-363.513303	-6.087390	8.064973
-361.522532	-2.039200	8.074970
-359.786144	-8.886249	8.084966
-357.878466	-4.414261	8.094963
-355.832660	-1.145384	8.104960
-354.206428	-2.240070	8.114957
-352.317491	-1.256159	8.124954
-350.333144	-0.759587	8.134950
-348.561977	2.704726	8.144947
-346.972615	0.979610	8.154944
-344.452946	-1.890353	8.164941
-342.776097	-4.366806	8.174938
-341.037649	-5.345188	8.184934
-339.115098	-2.067671	8.194931
-337.269492	-2.818420	8.204928
-335.096522	-0.902465	8.214925
-333.504130	-5.741760	8.224922
-331.661340	-2.107290	8.234918
-329.674796	-2.005791	8.244915
-327.798325	-3.765677	8.254912
-325.912446	-3.733368	8.264909
-323.963632	1.951039	8.274906
-322.315786	1.948720	8.284902
-320.722917	-2.150113	8.294899
-318.601264	-5.801251	8.304896
-316.616026	-3.422675	8.314893
-314.538392	-3.079914	8.324890
-312.949005	-6.685550	8.334886
-311.013471	-3.986402	8.344883
-309.115096	2.103967	8.354880
-307.278432	-2.935361	8.364877
-305.149823	-2.021252	8.374874
-303.348549	1.079866	8.384870
-301.713424	1.035381	8.394867
-299.678950	1.857153	8.404864
-297.541313	1.593504	8.414861
-296.076702	-3.541161	8.424858
-294.265949	-2.299984	8.434854
-292.414480	5.024738	8.444851
-290.452914	3.222875	8.454848
-288.345295	-4.294447	8.464845
-286.462120	0.688360	8.474842
-284.907003	2.714041	8.484838
-282.708681	-0.453513	8.494835
-280.700972	-0.513248	8.504832
-279.097996	0.540054	8.514829
-277.191602	-4.823017	8.524826
-275.341405	4.791413	8.534822
-273.527357	-4.689051	8.544819
-271.726968	-0.826710	8.554816
-269.396980	-2.373152	8.564813
-267.685941	5.147694	8.574810
-266.323570	5.137296	8.584807
-264.480868	2.934423	8.594803
-261.915094	-2.121779	8.604800
-260.254098	-4.864069	8.614797
-258.192229	-1.466616	8.624794
-256.503194	-7.200769	8.634791
-254.961517	-3.988704	8.644787
-252.883444	-6.540191	8.654784
-250.722479	-0.348001	8.664781
-248.929203	-2.487709	8.674778
-247.545884	-0.680900	8.684775
-245.169033	-9.753801	8.694771
-243.367874	-6.474197	8.704768
-241.403822	-1.087417	8.714765
-239.715887	-8.526659	8.724762
-237.751852	-1.799338	8.734759
-236.053521	-0.278065	8.744755
-234.036492	-1.067149	8.754752
-232.174707	-4.397262	8.764749
-230.283290	-8.226316	8.774746
-228.429577	-1.710328	8.784743
-226.455037	-6.950025	8.794739
-224.666695	-4.813107	8.804736
-222.443905	-2.876579	8.814733
-221.065064	-9.885948	8.824730
-219.174929	-1.675225	8.834727
-217.271540	-3.646167	8.844723
-215.267084	-2.205317	8.854720
-213.137053	-6.134021	8.864717
-211.333367	-8.488522	8.874714
-209.607045	-13.126481	8.884711
-207.801222	-11.251289	8.894707
-205.878011	-18.361736	8.904704
-204.055983	-16.315444	8.914701
-201.986056	-20.105068	8.924698
-200.245885	-12.266721	8.934695
-198.456592	-15.965766	8.944691
-196.643885	-11.966387	8.954688
-194.416486	-17.535361	8.964685
-192.659123	-14.641891	8.974682
-190.823091	-13.816778	8.984679
-189.203049	-11.090865	8.994675
-187.341737	-12.753487	9.004672
-185.240489	-15.534406	9.014669
-183.572066	-10.820405	9.024666
-181.570183	-7.176468	9.034663
-179.589653	-13.042352	9.044659
-177.774577	-13.473895	9.054656
-176.077157	-9.410310	9.064653
-173.706467	-14.610552	9.074650
-171.966560	-9.506895	9.084647
-170.327696	-9.063989	9.094643
-168.423196	-16.589849	9.104640
-166.543579	-19.659070	9.114637
-164.524649	-13.099924	9.124634
-162.746538	-12.688708	9.134631
-161.041212	-14.147995	9.144627
-158.840837	-12.387834	9.154624
-157.335521	-14.007835	9.164621
-155.313716	-14.057083	9.174618
-153.331782	-6.664645	9.184615
-151.406011	-9.065427	9.194611
-149.730636	-9.310445	9.204608
-147.870549	-18.142897	9.214605
-145.587376	-14.510658	9.224602
-143.945336	-14.687193	9.234599
-142.123398	-11.218195	9.244595
-140.188459	-11.234622	9.254592
-138.347455	-8.215507	9.264589
-136.369624	-11.485118	9.274586
-134.699887	-11.531855	9.284583
-132.722236	-8.280328	9.294579
-130.651295	-10.694784	9.304576
-129.226382	-5.919780	9.314573
-127.670005	-6.711063	9.324570
-125.141968	-12.247423	9.334567
-123.223491	-14.077013	9.344563
-121.207641	-5.553106	9.354560
-119.603039	-11.444227	9.364557
-117.530215	-10.236837	9.374554
-116.076028	-15.072892	9.384551
-113.888109	-9.347510	9.394547
-112.073190	-9.417397	9.404544
-110.226201	-7.477645	9.414541
-108.523234	-5.578070	9.424538
-106.530829	-1.893080	9.434535
-104.424831	-3.773104	9.444531
-102.824725	-5.013456	9.454528
-100.794576	-7.819278	9.464525
-98.958902	-7.000353	9.474522
-97.116059	-8.369432	9.484519
-95.210784	-0.686810	9.494515
-93.261859	-7.296017	9.504512
-91.308174	1.128892	9.514509
-89.549655	-4.298871	9.524506
-87.628210	-1.216759	9.534503
-85.856642	-1.672871	9.544499
-84.074141	-8.789207	9.554496
-81.799106	-15.840434	9.564493
-80.272298	-12.932201	9.574490
-78.364948	-6.795701	9.584487
-76.431820	-12.535523	9.594483
-74.923683	-9.617991	9.604480
-72.815221	-5.840961	9.614477
-70.724758	-8.050059	9.624474
-68.982834	-3.963493	9.634471
-67.157733	-7.432897	9.644467
-65.195455	-4.044646	9.654464
-63.043384	-5.657246	9.664461
-61.571056	-2.538199	9.674458
-59.571397	-5.080173	9.684455
-57.693654	-2.985811	9.694451
-55.665111	-3.553951	9.704448
-53.892819	-8.165983	9.714445
-51.870398	-5.540482	9.724442
-50.289484	-2.658226	9.734439
-48.313171	-6.587533	9.744435
-46.494351	-7.516948	9.754432
-44.552196	-4.027575	9.764429
-42.725864	-2.687637	9.774426
-40.950524	-1.787989	9.784423
-38.846082	2.723933	9.794419
-36.957701	-0.987653	9.804416
-35.185065	-2.043905	9.814413
-33.063073	0.693626	9.824410
-31.307475	-0.383589	9.834407
-29.616355	0.013182	9.844403
-27.603932	2.302402	9.854400
-25.763327	-5.292118	9.864397
-24.091297	-6.717580	9.874394
-22.072199	1.627483	9.884391
-20.339201	0.455985	9.894387
-18.174362	-8.301841	9.904384
-16.222184	-5.799316	9.914381
-14.750125	-3.959156	9.924378
-12.937224	-8.805009	9.934375
-10.553916	-6.521253	9.944371
-8.953770	-2.416761	9.954368
-6.956107	-0.744123	9.964365
-5.231249	14.415337	9.974362
-4.021774	37.842392	9.984359
-2.765684	70.884298	9.994355
-1.049203	114.866199	10.004352
0.000000	148.462215	10.009357
0.781062	184.024402	10.014362
1.352243	209.688412	10.019367
2.107434	228.988428	10.024371
2.209060	244.950192	10.029376
2.895770	264.466186	10.034381
2.942469	276.125301	10.039386
3.154776	279.717012	10.044391
3.437246	280.552018	10.049395
3.261732	288.657394	10.054400
3.633572	285.989875	10.059405
3.419149	291.409561	10.064410
3.553315	291.355155	10.069415
3.709272	294.033327	10.074419
3.292362	296.829686	10.079424
3.580642	297.491876	10.084429
3.303023	304.974872	10.089434
3.374240	306.606834	10.094439
3.624773	306.522827	10.099443
3.363718	306.165603	10.104448
3.718325	306.186423	10.109453
3.570774	305.208689	10.114458
3.426536	305.373735	10.119463
3.833218	301.691390	10.124467
3.375931	311.423432	10.129472
3.658776	325.252689	10.134477
3.900150	334.114776	10.139482
4.084709	336.603887	10.144487
4.471841	342.821787	10.149491
4.364047	351.872047	10.154496
4.733527	331.826556	10.159501
3.987569	331.441020	10.164506
4.138653	326.711323	10.169511
4.233977	334.964338	10.174515
4.276221	342.279635	10.179520
4.442263	337.076030	10.184525
4.610037	355.135789	10.189530
4.309437	340.727651	10.194535
4.837162	344.731122	10.199539
4.488900	345.829169	10.204544
4.816979	337.970888	10.209549
4.562136	342.991757	10.214554
4.486881	343.421772	10.219559
5.103742	355.373212	10.224563
4.567188	360.689762	10.229568
4.667645	356.236218	10.234573
4.916463	363.684158	10.239578
5.048385	371.962896	10.244583
5.157520	365.456308	10.249587
4.965596	372.533000	10.254592
5.214418	366.415722	10.259597
4.897260	362.300030	10.264602
5.074599	373.265013	10.269607
5.509164	369.258076	10.274611
5.121708	376.730243	10.279616
5.270794	375.028661	10.284621
5.091937	372.169841	10.289626
5.206657	373.227157	10.294631
5.375558	369.857119	10.299635
5.059608	378.702473	10.304640
5.427479	374.660440	10.309645
5.131371	384.261163	10.314650
5.552203	382.571429	10.319655
5.592597	384.061657	10.324659
5.505873	389.539860	10.329664
5.653084	385.747491	10.334669
5.411676	377.808136	10.339674
5.254566	388.843825	10.344679
5.300477	409.096177	10.349683
5.416360	420.719141	10.354688
5.674715	418.650033	10.359693
5.627677	423.170993	10.364698
5.723976	428.717790	10.369703
5.954367	420.941281	10.374707
5.972692	423.816477	10.379712
6.451481	432.938806	10.384717
6.414195	435.012301	10.389722
6.065702	425.360041	10.394727
6.235546	420.562664	10.399731
5.848670	433.316108	10.404736
6.429273	441.039181	10.409741
6.981936	454.115877	10.414746
6.560786	452.226115	10.419751
6.391598	432.249062	10.424755
6.370466	441.899004	10.429760
6.552862	446.436992	10.434765
6.677626	452.002913	10.439770
6.789173	460.335415	10.444775
7.030465	455.769487	10.449779
6.742148	447.397595	10.454784
6.540053	439.063996	10.459789
6.775802	450.292540	10.464794
6.744976	464.768067	10.469799
6.996772	460.314006	10.474803
7.014386	465.499621	10.479808
7.205648	472.633515	10.484813
7.166430	475.166229	10.489818
7.203035	486.096974	10.494823
7.296533	489.725036	10.499827
7.015865	500.581816	10.504832
7.008669	480.487391	10.509837
7.108028	483.863774	10.514842
7.114732	483.389717	10.519847
7.374600	479.033713	10.524851
7.170211	479.104274	10.529856
7.174898	477.988701	10.534861
7.028040	478.419102	10.539866
6.897603	472.461626	10.544871
7.442412	492.509933	10.549875
7.468945	505.140726	10.554880
7.879108	509.763044	10.559885
7.633043	511.338403	10.564890
7.614748	519.155469	10.569895
7.956801	517.257506	10.574899
7.707167	526.704248	10.579904
7.587257	510.959785	10.584909
7.817671	520.413532	10.589914
7.842070	516.552407	10.594919
8.137956	515.568584	10.599923
7.784115	525.106066	10.604928
7.928782	516.543640	10.609933
7.711956	525.595629	10.614938
7.999459	529.915023	10.619943
7.989648	540.903677	10.624947
8.187062	547.347476	10.629952
8.166416	551.328084	10.634957
8.417419	556.709901	10.639962
8.297897	555.169419	10.644967
8.739933	547.256578	10.649971
8.405080	562.540814	10.654976
8.721159	550.688202	10.659981
8.682913	555.447506	10.664986
8.537152	557.912070	10.669991
8.621445	556.995112	10.674995
8.722355	566.654057	10.680000
8.826528	562.737615	10.685005
8.643025	560.746852	10.690010
8.438283	563.815357	10.695015
8.864676	562.343920	10.700019
8.898626	556.339687	10.705024
9.103197	556.873313	10.710029
8.621320	563.152649	10.715034
8.805239	557.991848	10.720039
8.846266	557.291532	10.725043
8.948042	577.965731	10.730048
9.137589	581.537493	10.735053
9.279933	587.592688	10.740058
9.222938	598.568411	10.745063
9.333196	590.364681	10.750067
8.811663	601.252071	10.755072
9.217031	599.585280	10.760077
8.946050	599.458298	10.765082
9.163845	610.774989	10.770087
9.405110	609.955996	10.775091
9.405427	622.859165	10.780096
9.493915	616.819399	10.785101
9.665396	626.807761	10.790106
9.710151	630.322203	10.795111
9.909870	620.949812	10.800115
9.675725	632.813289	10.805120
9.770261	637.335389	10.810125
9.847223	632.734114	10.815130
9.898641	632.317578	10.820135
9.988768	631.191518	10.825139
9.754775	636.661764	10.830144
10.087192	629.646338	10.835149
10.117015	642.223107	10.840154
9.722553	641.797263	10.845159
10.295599	635.107743	10.850163
10.142251	645.367136	10.855168
10.239590	649.341568	10.860173
10.479869	642.623119	10.865178
10.251490	649.447129	10.870183
10.295617	646.516416	10.875187
10.314566	645.982050	10.880192
10.596972	659.266050	10.885197
10.893016	677.775701	10.890202
10.572039	664.632105	10.895207
10.559413	650.297578	10.900211
10.633695	670.714509	10.905216
10.815869	671.901443	10.910221
10.835960	672.101785	10.915226
10.848913	680.653575	10.920231
11.052887	675.931099	10.925235
11.005799	675.593354	10.930240
11.094078	664.942401	10.935245
11.162267	661.306075	10.940250
10.769500	658.307846	10.945255
11.039460	664.560346	10.950259
11.103451	678.380694	10.955264
11.237011	679.255247	10.960269
11.393546	679.839119	10.965274
11.215460	678.265385	10.970279
11.528370	672.456316	10.975283
11.462903	682.706448	10.980288
11.105094	680.983178	10.985293
11.467627	691.217089	10.990298
11.161294	686.703745	10.995303
11.481753	680.552832	11.000307
11.482235	680.876155	11.005312
11.468610	684.082941	11.010317
11.483501	687.231561	11.015322
11.414714	691.415437	11.020327
11.624987	688.246894	11.025331
11.699651	690.827715	11.030336
11.654671	679.898374	11.035341
11.505471	682.637909	11.040346
11.497041	706.327782	11.045351
12.237144	706.660870	11.050355
11.898027	720.996585	11.055360
11.939790	714.251417	11.060365
12.321566	718.757689	11.065370
12.209353	724.631185	11.070375
12.484634	720.360965	11.075379
12.289726	723.314389	11.080384
12.299841	709.042411	11.085389
12.465437	721.788412	11.090394
12.239602	717.356840	11.095399
12.730644	715.345197	11.100403
12.373794	715.862718	11.105408
12.217852	720.186666	11.110413
12.281821	721.712594	11.115418
12.419502	721.275987	11.120423
12.568815	721.708042	11.125427
12.550548	720.851589	11.130432
12.387461	723.672198	11.135437
12.474766	723.126926	11.140442
12.302876	728.189891	11.145447
12.416454	726.055520	11.150451
12.698308	741.415046	11.155456
12.540361	750.008330	11.160461
12.980960	749.225348	11.165466
12.857159	755.395608	11.170471
13.026159	748.190139	11.175475
12.819564	758.987986	11.180480
13.181938	749.744117	11.185485
13.022989	756.156538	11.190490
12.894710	754.316218	11.195495
13.316513	749.959538	11.200499
13.155303	757.331152	11.205504
13.131322	771.296513	11.210509
13.556187	778.327062	11.215514
13.306459	782.970355	11.220519
13.619370	779.634025	11.225523
13.309439	792.892775	11.230528
13.717375	781.192490	11.235533
13.872387	780.388823	11.240538
13.815840	788.216867	11.245543
14.105451	777.035378	11.250547
13.642674	772.840288	11.255552
13.703185	764.813136	11.260557
14.157523	782.670016	11.265562
13.571661	777.573572	11.270567
14.083679	778.308914	11.275571
14.051320	784.008840	11.280576
14.138262	770.453135	11.285581
14.309909	778.967055	11.290586
13.575209	766.373505	11.295591
14.049673	775.925694	11.300595
14.009060	781.803563	11.305600
14.155825	781.168377	11.310605
14.369920	780.844165	11.315610
14.315432	795.416841	11.320615
14.483492	787.173816	11.325619
14.191617	791.565201	11.330624
14.256888	786.188267	11.335629
14.396668	791.204694	11.340634
13.892340	790.786906	11.345639
14.130033	794.160221	11.350643
14.301367	814.243315	11.355648
14.609774	816.501433	11.360653
14.988320	819.748203	11.365658
15.014143	823.593734	11.370663
15.247532	819.929441	11.375667
15.104890	822.589104	11.380672
15.034210	804.981877	11.385677
15.067164	783.229477	11.390682
14.783366	792.640837	11.395687
14.669213	790.353537	11.400691
14.894248	807.975774	11.405696
15.373092	818.298462	11.410701
15.132123	821.994150	11.415706
15.226757	825.141119	11.420711
15.327647	818.810695	11.425715
15.314030	825.701461	11.430720
15.472073	824.007862	11.435725
15.369219	820.627447	11.440730
15.221508	835.899466	11.445735
15.372111	823.286087	11.450739
15.353984	825.914851	11.455744
15.272007	820.493579	11.460749
15.154338	827.232201	11.465754
15.275597	831.956691	11.470759
15.471969	825.201004	11.475763
15.407745	834.798153	11.480768
15.701501	843.231129	11.485773
15.748303	839.948272	11.490778
15.648954	852.216225	11.495783
15.715533	841.160153	11.500787
15.889154	856.548105	11.505792
15.728702	847.972648	11.510797
15.860539	850.232126	11.515802
15.486493	857.065274	11.520807
15.957328	846.238046	11.525811
15.924990	866.700647	11.530816
16.017040	877.461984	11.535821
16.401875	881.049983	11.540826
16.177608	882.861613	11.545831
16.535695	883.824953	11.550835
16.867242	879.386432	11.555840
16.743102	868.805484	11.560845
16.226445	862.396913	11.565850
16.204727	874.165198	11.570855
16.555726	868.608610	11.575859
16.710956	876.111170	11.580864
16.574469	883.004215	11.585869
16.698739	881.935773	11.590874
16.480486	884.497115	11.595879
16.760874	886.064238	11.600883
16.911322	879.853623	11.605888
17.104450	880.482132	11.610893
17.424349	872.735263	11.615898
16.833077	889.375991	11.620903
17.269843	875.928402	11.625907
16.963303	881.571168	11.630912
16.694933	881.161475	11.635917
16.790484	886.620253	11.640922
16.752905	884.200869	11.645927
16.922112	882.855585	11.650931
16.854811	887.250604	11.655936
16.885682	897.009254	11.660941
17.081423	902.310124	11.665946
17.008151	914.518774	11.670951
17.421827	912.631417	11.675955
17.663739	904.690378	11.680960
17.620729	912.965787	11.685965
17.649234	907.817036	11.690970
17.701053	912.961083	11.695975
17.634539	914.928914	11.700979
17.614421	913.176984	11.705984
17.324261	914.959702	11.710989
17.976191	908.388372	11.715994
17.414389	916.128331	11.720999
17.434942	913.165053	11.726003
17.543088	929.129684	11.731008
17.711699	941.017484	11.736013
18.291543	935.175197	11.741018
18.192202	935.099684	11.746023
18.518540	942.259577	11.751027
18.227778	948.648949	11.756032
18.575033	946.306953	11.761037
18.314778	928.666731	11.766042
17.900654	925.939950	11.771047
17.850368	930.444238	11.776051
18.403820	952.262828	11.781056
18.219468	949.072012	11.786061
18.323308	939.506540	11.791066
18.384970	946.998828	11.796071
18.100976	943.134737	11.801075
18.553088	948.360037	11.806080
18.586334	943.424995	11.811085
18.781451	939.812511	11.816090
18.481505	952.719708	11.821095
18.676986	946.088695	11.826099
18.896135	949.214254	11.831104
18.770589	949.390518	11.836109
18.532680	953.371196	11.841114
18.824176	965.239415	11.846119
19.191752	964.166854	11.851123
18.966379	976.276807	11.856128
19.075866	977.883817	11.861133
19.500907	980.978119	11.866138
19.217826	984.357269	11.871143
19.428604	974.277946	11.876147
19.397825	964.019526	11.881152
19.035267	959.597070	11.886157
19.476612	958.948008	11.891162
19.241878	975.378991	11.896167
19.590695	970.674320	11.901171
19.388691	976.965964	11.906176
19.220275	985.381273	11.911181
19.634672	979.947004	11.916186
19.497175	987.132013	11.921191
19.596827	977.750122	11.926195
19.479917	982.101039	11.931200
19.445783	984.323929	11.936205
19.530442	981.631126	11.941210
19.607839	987.474485	11.946215
20.062209	984.353681	11.951219
19.545504	987.863142	11.956224
19.667330	984.336458	11.961229
19.833318	978.009774	11.966234
19.892316	1004.334093	11.971239
20.066409	1004.221274	11.976243
20.325364	1011.150660	11.981248
20.056315	1016.691298	11.986253
20.292547	1018.596661	11.991258
19.803696	1014.421428	11.996263
20.161109	1006.559689	12.001267
20.162504	1014.129438	12.006272
20.347769	1008.186044	12.011277
20.646314	1005.681487	12.016282
20.077616	1007.824054	12.021287
20.383694	1008.699498	12.026291
20.584071	1008.216611	12.031296
20.654456	1011.123045	12.036301
20.734583	1005.434558	12.041306
20.581120	1012.152165	12.046311
20.728197	1003.656882	12.051315
20.437174	995.639940	12.056320
19.882492	979.013352	12.061325
20.556174	994.985629	12.066330
20.316017	1007.299828	12.071335
20.403819	1009.708289	12.076339
20.922377	1012.902808	12.081344
20.355970	996.777996	12.086349
20.305701	986.461164	12.091354
19.977015	984.961883	12.096359
20.618992	992.257547	12.101363
20.533641	988.243481	12.106368
20.108231	986.578266	12.111373
20.438516	984.063918	12.116378
20.285012	985.911585	12.121383
20.296513	985.569218	12.126387
20.552838	998.949160	12.131392
20.366695	996.001485	12.136397
20.341141	986.456621	12.141402
20.425453	987.988795	12.146407
20.403960	982.155666	12.151411
20.625234	988.229981	12.156416
20.433505	986.349287	12.161421
20.490986	976.751758	12.166426
20.331666	982.479897	12.171431
20.288613	980.955559	12.176435
20.226726	985.775547	12.181440
20.263972	980.945517	12.186445
20.762969	975.556107	12.191450
20.362492	981.731167	12.196455
20.536064	975.010589	12.201459
20.696460	978.391546	12.206464
20.558351	982.804196	12.211469
20.978755	985.534941	12.216474
20.958022	990.878256	12.221479
20.828912	984.122369	12.226483
20.454346	967.064918	12.231488
20.282405	966.024791	12.236493
20.073059	953.848781	12.241498
19.850741	963.794527	12.246503
20.185256	972.131186	12.251507
20.418597	980.882982	12.256512
20.492250	991.166338	12.261517
20.641706	985.231820	12.266522
20.557696	992.747367	12.271527
20.299777	982.657636	12.276531
20.598949	974.270583	12.281536
20.728057	972.042231	12.286541
20.501993	959.304299	12.291546
20.211613	968.808291	12.296551
20.405462	964.653497	12.301555
20.527693	960.514860	12.306560
20.316291	968.714652	12.311565
20.412554	963.234932	12.316570
20.372882	970.150425	12.321575
20.341866	957.785108	12.326579
20.330423	958.916211	12.331584
20.372627	965.069544	12.336589
20.415194	963.272915	12.341594
20.280609	969.744625	12.346599
20.322862	968.424314	12.351603
20.431116	959.572528	12.356608
20.165702	974.401391	12.361613
20.138732	964.536625	12.366618
20.400937	973.938288	12.371623
20.486144	970.415872	12.376627
20.296152	969.602565	12.381632
20.471879	974.411460	12.386637
20.825250	973.907325	12.391642
20.320331	973.117440	12.396647
20.412945	970.700932	12.401651
20.611991	971.000475	12.406656
20.255833	975.370627	12.411661
20.513347	970.921808	12.416666
20.068237	969.515219	12.421671
20.025538	968.687882	12.426675
20.325555	970.114681	12.431680
20.234726	976.868015	12.436685
20.558746	970.284302	12.441690
20.288307	979.165339	12.446695
20.168825	978.780783	12.451699
20.468597	967.018750	12.456704
20.109695	971.846683	12.461709
20.501052	981.598357	12.466714
20.738569	991.420311	12.471719
20.282666	975.542842	12.476723
20.607078	978.228968	12.481728
20.546550	977.290926	12.486733
20.798582	981.149307	12.491738
20.295208	984.181948	12.496743
20.567206	975.048553	12.501747
20.581030	978.582206	12.506752
20.763231	974.815646	12.511757
20.746563	970.301743	12.516762
20.591705	977.899550	12.521767
20.790583	977.222926	12.526771
20.394809	956.544808	12.531776
20.162016	956.468502	12.536781
20.353328	946.294526	12.541786
20.166306	954.542464	12.546791
20.246053	965.457227	12.551795
20.404085	981.049660	12.556800
20.059446	982.762223	12.561805
20.619930	979.143494	12.566810
20.511424	981.856093	12.571815
20.489366	975.644564	12.576819
20.883066	968.284868	12.581824
20.558631	961.575917	12.586829
20.743911	951.912286	12.591834
20.238241	951.026322	12.596839
20.308908	948.573891	12.601843
20.536499	946.310910	12.606848
20.291346	957.564512	12.611853
20.460286	947.999690	12.616858
20.398759	952.273952	12.621863
20.336329	954.217481	12.626867
20.193177	944.079507	12.631872
20.224847	963.726164	12.636877
20.801524	952.834664	12.641882
20.379825	955.409544	12.646887
20.256072	955.333194	12.651891
20.157746	963.581183	12.656896
19.968535	957.885209	12.661901
20.422433	956.713719	12.666906
19.995704	953.350238	12.671911
20.297969	951.371830	12.676915
20.360786	970.676040	12.681920
20.405150	983.417952	12.686925
20.848857	977.964816	12.691930
20.441926	968.026603	12.696935
20.134085	962.067257	12.701939
20.234103	953.363454	12.706944
20.727133	952.083215	12.711949
20.684122	951.729043	12.716954
20.437459	961.571430	12.721959
20.533651	957.432216	12.726963
20.761755	958.091422	12.731968
20.266565	963.519867	12.736973
20.687177	959.767326	12.741978
20.718631	962.481252	12.746983
20.498028	958.730056	12.751987
20.841309	961.186074	12.756992
20.392804	959.989775	12.761997
20.373222	951.260893	12.767002
20.303568	959.218861	12.772007
20.703499	954.745754	12.777011
20.655685	937.010132	12.782016
20.261270	935.232740	12.787021
20.269587	922.452725	12.792026
20.363255	932.001098	12.797031
20.191361	935.821422	12.802035
20.230023	936.244323	12.807040
20.466566	947.540941	12.812045
20.248755	928.465144	12.817050
20.151179	942.973874	12.822055
20.365224	957.535421	12.827059
20.684605	965.379297	12.832064
20.299639	961.614890	12.837069
20.815183	936.085530	12.842074
20.181527	936.784411	12.847079
20.312154	928.553586	12.852083
20.600630	919.111650	12.857088
20.210620	931.621586	12.862093
20.147361	931.122401	12.867098
20.175233	938.028682	12.872103
20.543309	948.533145	12.877107
20.796508	939.525780	12.882112
20.515415	938.656039	12.887117
20.190832	926.007972	12.892122
20.257241	948.501942	12.897127
19.984668	934.724291	12.902131
20.195436	939.456618	12.907136
20.154037	953.920126	12.912141
20.454695	954.376936	12.917146
20.398028	964.848228	12.922151
20.479665	961.802652	12.927155
20.638723	961.045642	12.932160
20.260330	969.514935	12.937165
20.550905	963.056415	12.942170
20.512307	953.549925	12.947175
20.190407	945.466968	12.952179
20.344057	947.972155	12.957184
20.234043	956.668309	12.962189
20.400970	957.550175	12.967194
20.252261	961.996050	12.972199
20.415002	967.986647	12.977203
20.624000	968.003887	12.982208
20.247446	960.125194	12.987213
20.465773	962.034982	12.992218
20.564675	957.488457	12.997223
20.484539	955.435416	13.002227
20.279739	940.071478	13.007232
19.877931	945.798855	13.012237
20.592358	955.514752	13.017242
20.598963	966.288208	13.022247
20.220826	948.479095	13.027251
20.470167	941.617129	13.032256
20.229503	941.138355	13.037261
20.498879	950.772262	13.042266
20.311327	946.261968	13.047271
20.130223	945.543446	13.052275
20.514973	957.907749	13.057280
20.453761	962.937370	13.062285
20.633993	952.290465	13.067290
20.445363	950.645838	13.072295
20.213068	944.884197	13.077299
20.167820	938.055027	13.082304
20.301964	954.086507	13.087309
20.757668	957.578061	13.092314
20.208263	950.215828	13.097319
20.257544	940.714254	13.102323
20.521780	938.409157	13.107328
20.093961	944.093370	13.112333
20.611944	951.855095	13.117338
20.586926	950.129175	13.122343
20.375508	947.256509	13.127347
20.338759	942.345248	13.132352
20.214702	940.262943	13.137357
20.373715	945.738431	13.142362
20.469793	941.771138	13.147367
20.241524	943.473020	13.152371
20.508589	938.114309	13.157376
20.430842	949.702346	13.162381
20.604277	939.491800	13.167386
20.410992	944.898893	13.172391
20.387352	948.482673	13.177395
20.406073	940.898932	13.182400
20.507906	950.405012	13.187405
20.502551	944.777494	13.192410
20.499171	944.789184	13.197415
20.495397	942.930558	13.202419
20.531459	939.895410	13.207424
20.587090	954.059573	13.212429
20.642162	949.344989	13.217434
20.636013	947.387388	13.222439
20.559831	949.206946	13.227443
20.784391	942.907207	13.232448
20.479763	941.941866	13.237453
20.157001	922.837082	13.242458
20.280627	920.283164	13.247463
20.408052	939.096028	13.252467
20.571144	933.460572	13.257472
19.903134	927.031955	13.262477
20.020677	941.091608	13.267482
20.352439	944.970380	13.272487
20.268231	954.020406	13.277491
20.602719	935.274425	13.282496
20.361063	948.628088	13.287501
20.446703	938.284880	13.292506
20.447030	952.405821	13.297511
20.643924	953.500539	13.302515
20.445969	952.421982	13.307520
20.110307	955.328512	13.312525
20.421470	946.032760	13.317530
20.275984	946.828830	13.322535
20.228794	957.737024	13.327539
20.750853	951.926026	13.332544
20.766696	957.332885	13.337549
20.509124	938.086788	13.342554
20.307872	927.208996	13.347559
20.263297	927.992123	13.352563
20.219015	920.932559	13.357568
20.292090	940.722400	13.362573
20.220893	938.688437	13.367578
20.430061	947.078193	13.372583
20.359586	952.580826	13.377587
20.542147	955.664911	13.382592
20.598357	947.993180	13.387597
20.397734	933.697821	13.392602
20.321446	931.980081	13.397607
20.138779	929.930781	13.402611
20.562476	919.038474	13.407616
20.333414	926.872031	13.412621
20.366651	920.719519	13.417626
20.262739	920.170046	13.422631
20.308016	927.830527	13.427635
20.407742	925.734609	13.432640
20.635692	926.625664	13.437645
20.410518	918.703923	13.442650
20.458600	919.648899	13.447655
20.271301	928.317937	13.452659
20.353193	923.652703	13.457664
20.140800	929.655807	13.462669
20.210307	928.960394	13.467674
20.588215	935.662600	13.472679
19.923252	936.948405	13.477683
20.256426	946.083249	13.482688
20.544234	956.146331	13.487693
20.308951	961.077552	13.492698
20.381687	964.120806	13.497703
20.518776	958.429560	13.502707
20.801589	951.402968	13.507712
20.610026	941.871996	13.512717
20.474139	933.056013	13.517722
20.227386	929.474585	13.522727
20.587314	933.829860	13.527731
20.508452	929.846316	13.532736
20.412665	936.713970	13.537741
20.547271	931.086212	13.542746
20.511375	927.348143	13.547751
20.385234	937.053012	13.552755
20.516946	928.411981	13.557760
20.223166	938.137282	13.562765
20.071285	941.225820	13.567770
20.323734	924.722883	13.572775
20.394179	926.306150	13.577779
20.704971	931.134490	13.582784
20.210057	931.213541	13.587789
20.620920	933.602002	13.592794
20.480230	933.296528	13.597799
20.377470	937.165753	13.602803
20.593516	930.203441	13.607808
20.292144	931.702504	13.612813
20.242518	933.973591	13.617818
20.632560	933.387910	13.622823
20.195556	939.426845	13.627827
20.460334	936.300020	13.632832
20.606965	928.479828	13.637837
20.438894	926.507053	13.642842
20.471094	930.556612	13.647847
20.290846	939.637718	13.652851
20.534372	934.189717	13.657856
20.248961	936.164079	13.662861
20.457674	937.845149	13.667866
20.316151	940.034696	13.672871
20.290234	939.671489	13.677875
20.613697	941.329525	13.682880
20.434167	943.157682	13.687885
20.477749	934.891849	13.692890
20.406659	941.326609	13.697895
20.191162	942.170117	13.702899
20.336191	940.475426	13.707904
20.158756	940.363481	13.712909
20.046024	937.150205	13.717914
20.147624	942.076575	13.722919
20.013423	944.269685	13.727923
20.159688	935.769840	13.732928
20.094060	943.791816	13.737933
20.354154	948.995701	13.742938
20.516571	943.147447	13.747943
20.268273	938.208426	13.752947
20.338253	938.030208	13.757952
20.181828	940.605353	13.762957
20.146393	944.799753	13.767962
20.388313	941.783812	13.772967
20.116838	947.302732	13.777971
20.197613	957.892453	13.782976
20.360574	979.577816	13.787981
20.486354	979.925318	13.792986
20.885187	966.020043	13.797991
20.313547	960.292021	13.802995
20.284741	947.044791	13.808000
20.349853	949.310196	13.813005
20.379345	947.599237	13.818010
20.617658	940.185487	13.823015
20.329395	944.016490	13.828019
20.332349	939.362264	13.833024
20.405341	938.319344	13.838029
20.529607	942.193363	13.843034
20.453602	942.511544	13.848039
20.361719	945.929578	13.853043
20.558306	943.791398	13.858048
20.531736	945.648777	13.863053
20.644804	940.598497	13.868058
20.655243	949.261240	13.873063
20.373194	947.376032	13.878067
20.617333	933.601125	13.883072
20.525806	953.740533	13.888077
20.867854	948.199537	13.893082
20.817985	944.673439	13.898087
20.420317	937.961986	13.903091
20.445134	919.908853	13.908096
20.333810	931.822372	13.913101
20.298215	922.697068	13.918106
20.540353	923.051242	13.923111
20.580596	919.845110	13.928115
20.434618	926.318618	13.933120
20.413693	929.487197	13.938125
20.342060	933.045509	13.943130
20.511184	923.199960	13.948135
20.292003	932.091718	13.953139
20.404746	931.231703	13.958144
20.205071	926.595608	13.963149
20.341776	935.047381	13.968154
20.405354	926.075001	13.973159
20.140087	933.285095	13.978163
20.545231	928.309664	13.983168
20.352908	937.192409	13.988173
20.083678	925.748262	13.993178
20.430142	927.077757	13.998183
20.225095	935.513073	14.003187
20.323709	927.703694	14.008192
20.107918	932.111390	14.013210
20.435661	935.873806	14.018227
20.472499	942.603729	14.023245
20.036083	949.431162	14.028263
20.452482	950.450243	14.033280
20.347368	953.361486	14.038298
20.353332	953.989856	14.043315
20.610425	945.509683	14.048333
20.310385	955.997817	14.053351
20.622829	957.115278	14.058368
20.477032	954.028773	14.063386
20.469497	957.893436	14.068403
20.555123	953.420363	14.073421
20.534355	956.429838	14.078439
20.714109	947.073241	14.083456
20.578883	950.105690	14.088474
20.417639	951.978251	14.093491
20.557891	947.133098	14.098509
20.488416	956.302441	14.103527
20.627789	950.329569	14.108544
20.577926	955.610413	14.113562
20.696641	955.111816	14.118579
20.994064	953.165847	14.123597
20.815909	956.063572	14.128615
20.909303	953.349475	14.133632
20.823501	958.972681	14.138650
20.859936	955.245202	14.143667
20.933331	960.695151	14.148685
20.871394	963.363556	14.153703
20.702850	955.390141	14.158720
20.987487	974.044989	14.163738
20.573014	963.609683	14.168755
20.882616	955.506520	14.173773
20.669923	965.235115	14.178791
21.199568	953.312155	14.183808
21.033036	966.885727	14.188826
20.650200	971.233399	14.193843
21.184279	971.039784	14.198861
20.794731	994.165769	14.203879
20.996455	995.793251	14.208896
21.283060	991.791479	14.213914
21.048965	993.362633	14.218931
21.222979	997.623067	14.223949
21.152563	1000.840245	14.228967
21.390190	992.342700	14.233984
21.295519	989.266910	14.239002
20.826930	991.957709	14.244019
21.590425	983.583932	14.249037
21.252719	993.337204	14.254055
21.109756	992.104841	14.259072
21.432099	1004.052610	14.264090
21.239108	997.454755	14.269107
21.315239	990.151731	14.274125
21.122419	1005.431549	14.279143
20.936963	999.714961	14.284160
21.239910	999.237315	14.289178
21.271455	1001.689467	14.294195
21.529724	1001.269284	14.299213
21.198226	1007.765403	14.304231
21.153145	1004.570014	14.309248
21.432980	998.529100	14.314266
21.089076	1005.376409	14.319283
21.316562	997.486096	14.324301
21.304539	1008.151698	14.329319
21.286725	1001.765000	14.334336
21.638264	1003.911283	14.339354
21.486676	1003.447933	14.344371
22.100630	1008.904489	14.349389
21.638036	1016.035004	14.354407
21.733295	1010.495435	14.359424
21.706723	1002.622046	14.364442
21.623807	1006.330431	14.369459
21.729080	994.226588	14.374477
21.688389	1006.515409	14.379495
21.606070	1004.401913	14.384512
21.703872	1002.387103	14.389530
21.580587	1004.543053	14.394547
21.505982	1003.038663	14.399565
21.471783	1027.627569	14.404583
21.616890	1031.414422	14.409600
21.679958	1038.986497	14.414618
21.768559	1036.155172	14.419635
21.992458	1039.850808	14.424653
21.833559	1030.788847	14.429671
21.958688	1034.100685	14.434688
22.108940	1031.324022	14.439706
21.880907	1038.465899	14.444723
21.966251	1036.880937	14.449741
21.909650	1037.612099	14.454759
21.793729	1039.678790	14.459776
21.746919	1037.872659	14.464794
21.856573	1037.576853	14.469811
22.047836	1036.610503	14.474829
22.135474	1043.848324	14.479847
21.998937	1037.796727	14.484864
21.939357	1040.582747	14.489882
21.746176	1040.420188	14.494899
22.095712	1030.844546	14.499917
21.842821	1059.663669	14.504935
22.126546	1066.176516	14.509952
22.764320	1066.290407	14.514970
22.289175	1061.689666	14.519987
22.412834	1037.715869	14.525005
22.471015	1039.164903	14.530023
22.010728	1039.109443	14.535040
22.391782	1042.039113	14.540058
22.260324	1046.739971	14.545075
22.456625	1045.519558	14.550093
22.322679	1041.690244	14.555111
22.564992	1054.380708	14.560128
22.400414	1036.704133	14.565146
22.353146	1042.970888	14.570163
22.455240	1039.374488	14.575181
22.471017	1044.811637	14.580199
22.724425	1051.758752	14.585216
22.967080	1033.188238	14.590234
22.527362	1032.707923	14.595251
22.934540	1021.885116	14.600269
22.683043	1028.912753	14.605287
22.416157	1032.202174	14.610304
22.775293	1030.219610	14.615322
22.381043	1032.178110	14.620339
22.700295	1032.825727	14.625357
22.544787	1032.152215	14.630375
22.202349	1031.854586	14.635392
22.598124	1037.076964	14.640410
22.540552	1056.495939	14.645427
23.080203	1061.399646	14.650445
22.988078	1044.627013	14.655463
22.764811	1040.855992	14.660480
22.771193	1035.931488	14.665498
22.637988	1039.589701	14.670515
22.887595	1042.458540	14.675533
22.986634	1052.098145	14.680551
22.685331	1048.504737	14.685568
23.245279	1048.481603	14.690586
22.964629	1038.188494	14.695603
23.062561	1028.601075	14.700621
23.020736	1030.309879	14.705639
22.591600	1028.553720	14.710656
22.998887	1040.931566	14.715674
22.769481	1055.070529	14.720691
23.030926	1055.991638	14.725709
23.097125	1056.360292	14.730727
23.240669	1064.978198	14.735744
23.532943	1054.853246	14.740762
23.184240	1057.896171	14.745779
23.214462	1053.744939	14.750797
23.280818	1035.429059	14.755815
23.071751	1027.358248	14.760832
23.393102	1037.125979	14.765850
23.121482	1034.059526	14.770867
23.280784	1039.708162	14.775885
23.471346	1043.495633	14.780903
23.085929	1050.514754	14.785920
23.345900	1043.830472	14.790938
23.007066	1049.138565	14.795955
23.186742	1050.972492	14.800973
23.469136	1052.127787	14.805991
23.568137	1049.529183	14.811008
23.615683	1054.794526	14.816026
23.387914	1060.301987	14.821043
23.385112	1054.535794	14.826061
23.548910	1057.062817	14.831079
23.152245	1055.298329	14.836096
23.581429	1057.867967	14.841114
23.225120	1066.285600	14.846131
23.555108	1069.116456	14.851149
23.527091	1058.512474	14.856167
23.600447	1060.335046	14.861184
23.406742	1058.503578	14.866202
23.558064	1063.945856	14.871219
23.569740	1060.838930	14.876237
23.686078	1055.338453	14.881255
23.155576	1069.427927	14.886272
23.656843	1061.165146	14.891290
23.506174	1061.765021	14.896307
23.362167	1067.031034	14.901325
23.699120	1080.216089	14.906343
23.886140	1083.222336	14.911360
23.777369	1084.290586	14.916378
23.947959	1087.595186	14.921395
23.978909	1082.341128	14.926413
24.055533	1089.052188	14.931431
23.882706	1085.101649	14.936448
24.020145	1083.292865	14.941466
24.008245	1082.703412	14.946483
23.924617	1083.800686	14.951501
24.111543	1080.801085	14.956519
24.053360	1081.468007	14.961536
24.191459	1084.809248	14.966554
24.349563	1084.897401	14.971571
24.099609	1082.203438	14.976589
24.024817	1071.141288	14.981607
24.078258	1087.151128	14.986624
24.418578	1080.480755	14.991642
24.279215	1075.017910	14.996659
23.923887	1075.798294	15.001677
24.089508	1076.792890	15.006695
23.812994	1086.058260	15.011712
24.477509	1083.791024	15.016730
24.446193	1084.334110	15.021747
24.137199	1096.077484	15.026765
24.114047	1087.940806	15.031783
24.051550	1090.225501	15.036800
24.149895	1088.621156	15.041818
24.173674	1096.691890	15.046835
23.893758	1088.973695	15.051853
24.208029	1079.957356	15.056871
24.130679	1093.677271	15.061888
24.298341	1112.487808	15.066906
24.329960	1117.288521	15.071923
24.433450	1118.956855	15.076941
24.714263	1107.754587	15.081959
24.676114	1133.407678	15.086976
24.803414	1121.138192	15.091994
25.295660	1119.172138	15.097011
24.855207	1113.647189	15.102029
24.827135	1089.596833	15.107047
24.593526	1086.733520	15.112064
24.673204	1085.127434	15.117082
24.554412	1087.850548	15.122099
24.791486	1078.969219	15.127117
24.789456	1076.953019	15.132135
24.819981	1089.560889	15.137152
24.821179	1088.802604	15.142170
25.022667	1094.485432	15.147187
25.161244	1088.496900	15.152205
25.020496	1106.038414	15.157223
24.843822	1111.603812	15.162240
24.970616	1108.709752	15.167258
25.304430	1103.290975	15.172275
24.862455	1104.989679	15.177293
25.377851	1101.154308	15.182311
25.110377	1100.407415	15.187328
25.027862	1105.965658	15.192346
25.275398	1100.909858	15.197363
25.171943	1107.449873	15.202381
25.298678	1105.875605	15.207399
25.311262	1107.542706	15.212416
25.073461	1091.351684	15.217434
24.952042	1083.296750	15.222451
24.852117	1082.029199	15.227469
24.854716	1079.148662	15.232487
24.647759	1090.015305	15.237504
24.694785	1091.148369	15.242522
25.070517	1084.936393	15.247539
25.183835	1104.919638	15.252557
25.543241	1106.229397	15.257575
25.461654	1115.300098	15.262592
25.462535	1102.723598	15.267610
25.481913	1099.016107	15.272627
24.888618	1100.013775	15.277645
25.391322	1100.651011	15.282663
25.170365	1110.590235	15.287680
25.098246	1113.925687	15.292698
25.158208	1115.136916	15.297715
25.071466	1111.111289	15.302733
25.068202	1109.735510	15.307751
25.352990	1117.107092	15.312768
25.724848	1136.445095	15.317786
25.432877	1142.068221	15.322803
25.541812	1149.016404	15.327821
26.115295	1135.882924	15.332839
26.043999	1141.658044	15.337856
25.843552	1134.049847	15.342874
25.795333	1115.929895	15.347891
25.504934	1114.250697	15.352909
25.611059	1108.239017	15.357927
25.366501	1124.422273	15.362944
25.595444	1142.620600	15.367962
25.834813	1145.022326	15.372979
25.690009	1152.721999	15.377997
26.060657	1146.838001	15.383015
26.149167	1145.379939	15.388032
25.862631	1147.686220	15.393050
26.159473	1138.027676	15.398067
26.092422	1142.290423	15.403085
26.140290	1143.379312	15.408103
26.274326	1138.122950	15.413120
25.961035	1136.692796	15.418138
26.279504	1142.229568	15.423155
26.017516	1144.236200	15.428173
26.209338	1136.282287	15.433191
26.327192	1138.325862	15.438208
25.949509	1132.385048	15.443226
26.139445	1128.518210	15.448243
26.366978	1137.786588	15.453261
26.072726	1138.255208	15.458279
26.419973	1144.462227	15.463296
26.342339	1145.083490	15.468314
26.518608	1138.558809	15.473331
25.933515	1135.731098	15.478349
26.021965	1135.592831	15.483367
26.174809	1141.193773	15.488384
26.302782	1145.123390	15.493402
26.425998	1137.812782	15.498419
26.220520	1148.893167	15.503437
26.331074	1152.160165	15.508455
26.407541	1145.582185	15.513472
26.665452	1140.798427	15.518490
26.351643	1141.383427	15.523507
26.252654	1144.844296	15.528525
26.511346	1138.877484	15.533543
26.709597	1145.779959	15.538560
26.445722	1146.954751	15.543578
26.751933	1137.861010	15.548595
26.661378	1143.300998	15.553613
26.408082	1144.434777	15.558631
26.440973	1158.377845	15.563648
26.810699	1171.112584	15.568666
27.278201	1170.983072	15.573683
26.777473	1171.915642	15.578701
26.689368	1152.737051	15.583719
27.056549	1168.097608	15.588736
26.641277	1163.765713	15.593754
26.824542	1165.087842	15.598771
27.001234	1178.830239	15.603789
26.901137	1169.211391	15.608807
26.865954	1174.383006	15.613824
26.788333	1177.444067	15.618842
26.963846	1170.836120	15.623859
26.906969	1181.820467	15.628877
27.035292	1179.072443	15.633895
27.078488	1172.482454	15.638912
26.709738	1175.140057	15.643930
26.934047	1179.455446	15.648947
26.541893	1178.220340	15.653965
26.609690	1174.940841	15.658983
27.321533	1193.222660	15.664000
27.132593	1206.301371	15.669018
27.198799	1194.364044	15.674035
27.373601	1202.361984	15.679053
27.628086	1204.001524	15.684071
27.576963	1209.957501	15.689088
27.616668	1191.439606	15.694106
27.752857	1189.072576	15.699123
27.259306	1181.586610	15.704141
26.999189	1174.607691	15.709159
27.572772	1178.548041	15.714176
27.062220	1191.902982	15.719194
27.594220	1191.209469	15.724211
27.403798	1204.071333	15.729229
27.525711	1206.115844	15.734247
27.810489	1202.443075	15.739264
27.566451	1210.454340	15.744282
28.001061	1198.673757	15.749299
27.911341	1205.307581	15.754317
27.764505	1192.715239	15.759335
27.702593	1173.203676	15.764352
27.704291	1175.377470	15.769370
27.499118	1172.465559	15.774387
27.708982	1191.289917	15.779405
27.737719	1205.378414	15.784423
27.943764	1198.015239	15.789440
27.762758	1202.760230	15.794458
28.034033	1197.409596	15.799475
27.946669	1201.703916	15.804493
27.914864	1205.446672	15.809511
27.562117	1202.300312	15.814528
27.645033	1208.090188	15.819546
28.089206	1199.038899	15.824563
28.000932	1201.020978	15.829581
27.750293	1196.895625	15.834599
28.017420	1202.750501	15.839616
27.690038	1200.526623	15.844634
28.070054	1198.905655	15.849651
28.021557	1204.571769	15.854669
27.838339	1205.288527	15.859687
28.284921	1212.266258	15.864704
28.124789	1234.575797	15.869722
28.326994	1239.181025	15.874739
28.416205	1239.122862	15.879757
28.209266	1231.504637	15.884775
28.728578	1234.053640	15.889792
28.331405	1242.874302	15.894810
28.331464	1225.394612	15.899827
28.512345	1231.562136	15.904845
28.125340	1236.047406	15.909863
28.715270	1231.215381	15.914880
28.589899	1234.062269	15.919898
28.576339	1232.298002	15.924915
28.364246	1231.259119	15.929933
28.824249	1224.053630	15.934951
29.104030	1225.495652	15.939968
28.546804	1219.783217	15.944986
28.582735	1209.442637	15.950003
28.652189	1207.344230	15.955021
28.513780	1207.808445	15.960039
28.877398	1218.736762	15.965056
28.412377	1222.131761	15.970074
28.598674	1227.472566	15.975091
28.788207	1226.681088	15.980109
28.514942	1234.698601	15.985127
29.132446	1231.134780	15.990144
28.715232	1229.735350	15.995162
28.904720	1229.011520	16.000179
29.049230	1221.417471	16.005197
28.838369	1230.810889	16.010215
29.097334	1231.817351	16.015232
28.991253	1231.263363	16.020250
28.869956	1235.316135	16.025267
28.985593	1218.585669	16.030285
28.836002	1239.680710	16.035303
29.256012	1230.350106	16.040320
28.757149	1238.285625	16.045338
29.010878	1234.926119	16.050355
29.222136	1229.504820	16.055373
28.953108	1233.560705	16.060391
29.142102	1227.438230	16.065408
29.107310	1239.395965	16.070426
29.269472	1249.330806	16.075443
29.585253	1245.423415	16.080461
29.141287	1257.498338	16.085479
29.256255	1250.390342	16.090496
29.164862	1264.476033	16.095514
29.464913	1263.495463	16.100531
29.529292	1256.787224	16.105549
29.508524	1259.793615	16.110567
29.574346	1255.819122	16.115584
29.472694	1262.082061	16.120602
29.730379	1261.341060	16.125619
29.769115	1250.439995	16.130637
29.723838	1264.755863	16.135655
29.649233	1258.324627	16.140672
29.550354	1255.466532	16.145690
29.277825	1256.217988	16.150707
29.554539	1253.699544	16.155725
29.642597	1252.928969	16.160743
29.854878	1252.110266	16.165760
29.634731	1254.662382	16.170778
29.648518	1250.818888	16.175795
29.676487	1247.622806	16.180813
29.819041	1255.292430	16.185831
29.935388	1242.406378	16.190848
29.783945	1252.778212	16.195866
29.683966	1260.197080	16.200883
30.117162	1273.936409	16.205901
30.175489	1276.398494	16.210919
30.359074	1277.243945	16.215936
30.182246	1264.583963	16.220954
30.208155	1250.982429	16.225971
30.400980	1248.897372	16.230989
29.868727	1248.383042	16.236007
30.199690	1244.841325	16.241024
30.200524	1253.243001	16.246042
29.825868	1256.228757	16.251059
30.161894	1261.004561	16.256077
30.396421	1278.134061	16.261095
30.450974	1282.624424	16.266112
30.680596	1278.900657	16.271130
30.476428	1263.389933	16.276147
30.601105	1251.411771	16.281165
30.191658	1254.223747	16.286183
30.229280	1249.932850	16.291200
30.447185	1270.108857	16.296218
30.477998	1278.593858	16.301235
30.674895	1277.717831	16.306253
30.769316	1278.376152	16.311271
30.379196	1282.651143	16.316288
30.519469	1285.169374	16.321306
30.502622	1283.465401	16.326323
30.840443	1275.684758	16.331341
30.752642	1294.166609	16.336359
30.722873	1282.524522	16.341376
30.631171	1282.319031	16.346394
30.699679	1287.804491	16.351411
30.728319	1283.592095	16.356429
30.453798	1291.046684	16.361447
30.927884	1280.961791	16.366464
30.763863	1289.482593	16.371482
30.538971	1288.153157	16.376499
30.999007	1279.678175	16.381517
30.444892	1282.768067	16.386535
30.865167	1281.653486	16.391552
31.250176	1298.305967	16.396570
31.247403	1303.565269	16.401587
31.506201	1302.371048	16.406605
31.099736	1292.052205	16.411623
31.548582	1273.478387	16.416640
31.568718	1274.773061	16.421658
31.132206	1274.312673	16.426675
31.083220	1274.569141	16.431693
31.045884	1283.002092	16.436711
31.097216	1272.695190	16.441728
31.357328	1291.648522	16.446746
31.401939	1300.134480	16.451763
31.465654	1301.812325	16.456781
31.457940	1307.177811	16.461799
31.923001	1294.783519	16.466816
31.295040	1290.458767	16.471834
31.285680	1283.559351	16.476851
31.611726	1296.084085	16.481869
31.536184	1305.828784	16.486887
31.712774	1308.666851	16.491904
31.915987	1296.993885	16.496922
31.569001	1293.712875	16.501939
31.699058	1279.734471	16.506957
31.630484	1293.681268	16.511975
31.770717	1293.802161	16.516992
31.900074	1288.263340	16.522010
31.310057	1300.238895	16.527027
32.243355	1288.031054	16.532045
32.523176	1288.194179	16.537063
32.063658	1273.392722	16.542080
32.083310	1270.499988	16.547098
31.768027	1267.149433	16.552115
32.261167	1263.868141	16.557133
31.796308	1269.459115	16.562151
31.899554	1269.046347	16.567168
32.018713	1271.580528	16.572186
32.172660	1266.910841	16.577203
32.115223	1255.372292	16.582221
32.045711	1260.901778	16.587239
31.666828	1267.822429	16.592256
32.172632	1273.639266	16.597274
32.125384	1286.020606	16.602291
32.404051	1290.391854	16.607309
32.227810	1297.747397	16.612327
32.294399	1306.140189	16.617344
32.580518	1289.380878	16.622362
32.072774	1298.455168	16.627379
32.250175	1295.145577	16.632397
32.131511	1293.973806	16.637415
32.066252	1291.829232	16.642432
32.186228	1293.125287	16.647450
32.203475	1298.796682	16.652467
32.081652	1298.723413	16.657485
31.944990	1312.523782	16.662503
32.298767	1315.009538	16.667520
32.397778	1321.013975	16.672538
32.361610	1330.135769	16.677555
32.624773	1321.102265	16.682573
33.032685	1320.280671	16.687591
32.882566	1322.492859	16.692608
32.812424	1328.974176	16.697626
32.937155	1331.677370	16.702643
33.234776	1327.009917	16.707661
32.887988	1329.574380	16.712679
33.041292	1323.419803	16.717696
33.127850	1328.616101	16.722714
32.814177	1321.590595	16.727731
33.135373	1326.710142	16.732749
32.905634	1320.420028	16.737767
32.910283	1323.043270	16.742784
33.270209	1317.445640	16.747802
32.931735	1324.630440	16.752819
32.963447	1319.454828	16.757837
32.965425	1327.352984	16.762855
33.148146	1341.811892	16.767872
33.871818	1334.845874	16.772890
33.362158	1334.516705	16.777907
33.507326	1314.863381	16.782925
33.410542	1317.435158	16.787943
33.374412	1320.349629	16.792960
33.196124	1317.276093	16.797978
33.078128	1321.241844	16.802995
33.145922	1314.281343	16.808013
33.659424	1340.419408	16.813031
33.734307	1346.086349	16.818048
33.952168	1339.282804	16.823066
33.784677	1338.296574	16.828083
33.518057	1316.552253	16.833101
33.350770	1320.176644	16.838119
33.401114	1331.046473	16.843136
33.876799	1334.543147	16.848154
33.480456	1344.543537	16.853171
34.121574	1339.671852	16.858189
34.001489	1344.341103	16.863207
33.505747	1353.669923	16.868224
33.819204	1342.229455	16.873242
33.838954	1341.650674	16.878259
33.979297	1341.606378	16.883277
33.845200	1350.289187	16.888295
33.876814	1347.721728	16.893312
34.016047	1338.291117	16.898330
33.848447	1346.079473	16.903347
33.833211	1344.394113	16.908365
33.843487	1332.341321	16.913383
33.545131	1348.841727	16.918400
34.401616	1344.808743	16.923418
34.199597	1353.091816	16.928435
33.961016	1352.816940	16.933453
34.475162	1359.535422	16.938471
34.359581	1374.598808	16.943488
34.517148	1361.989228	16.948506
34.356576	1365.277496	16.953523
34.503686	1363.591410	16.958541
34.841723	1354.269083	16.963559
34.421893	1349.426610	16.968576
34.834985	1335.845041	16.973594
34.330893	1333.221452	16.978611
34.245151	1335.052130	16.983629
34.317114	1353.753973	16.988647
34.312048	1364.945705	16.993664
34.775949	1370.313075	16.998682
34.784481	1371.971414	17.003699
34.957292	1369.471096	17.008717
34.988007	1370.726338	17.013735
34.684271	1379.387456	17.018752
34.740973	1369.556271	17.023770
34.614347	1369.376798	17.028787
34.919341	1370.762904	17.033805
34.901321	1359.765413	17.038823
35.015271	1368.965537	17.043840
35.045187	1367.741748	17.048858
35.039979	1372.999890	17.053875
35.076788	1367.482093	17.058893
35.282751	1366.409555	17.063911
34.768044	1376.177154	17.068928
35.400232	1367.627472	17.073946
35.512344	1371.004387	17.078963
35.523520	1373.576259	17.083981
34.950981	1368.885555	17.088999
35.108737	1367.059339	17.094016
35.349150	1362.984609	17.099034
35.259333	1361.149116	17.104051
35.010530	1362.831195	17.109069
35.106891	1364.244284	17.114087
35.036053	1366.860697	17.119104
35.239352	1359.983958	17.124122
35.257438	1353.316092	17.129139
35.355140	1377.296225	17.134157
35.426379	1378.647253	17.139175
35.382759	1381.839791	17.144192
35.844517	1389.229693	17.149210
35.588900	1384.014154	17.154227
35.671986	1382.173104	17.159245
36.051150	1378.186354	17.164263
35.796134	1385.590687	17.169280
35.694742	1382.843083	17.174298
36.159375	1383.418766	17.179315
36.007371	1384.791243	17.184333
36.005517	1381.277408	17.189351
35.565646	1384.655847	17.194368
35.610696	1380.179677	17.199386
35.437363	1386.812762	17.204403
35.601484	1386.412305	17.209421
36.191470	1381.544043	17.214439
35.856696	1379.421992	17.219456
36.148072	1382.998413	17.224474
36.139281	1383.844666	17.229491
35.848863	1388.312217	17.234509
36.105846	1399.720950	17.239527
36.155760	1411.243733	17.244544
36.486424	1418.018250	17.249562
36.306004	1418.168264	17.254579
36.177997	1417.619339	17.259597
36.433212	1404.649644	17.264615
36.203369	1420.648404	17.269632
36.384651	1415.156311	17.274650
36.451597	1419.321473	17.279667
36.059564	1415.401872	17.284685
36.320339	1413.686638	17.289703
36.593021	1417.299871	17.294720
36.789469	1418.346993	17.299738
36.523325	1420.469945	17.304755
36.459397	1428.604404	17.309773
36.564746	1415.170949	17.314791
36.707355	1423.998438	17.319808
36.910810	1440.257669	17.324826
37.161406	1441.668976	17.329843
36.833651	1435.057020	17.334861
36.984295	1416.951379	17.339879
36.874979	1418.829874	17.344896
36.928875	1412.021772	17.349914
37.006194	1412.770133	17.354931
36.738898	1428.936902	17.359949
37.234912	1431.167964	17.364967
36.952150	1443.708916	17.369984
37.053970	1439.313338	17.375002
37.261479	1451.891722	17.380019
37.238437	1438.663560	17.385037
37.522255	1438.936952	17.390055
37.285397	1447.111587	17.395072
37.071229	1446.736070	17.400090
37.543075	1442.539459	17.405107
37.171760	1446.581041	17.410125
37.381862	1434.320895	17.415143
37.327117	1444.530360	17.420160
37.150676	1439.878706	17.425178
37.350977	1436.320817	17.430195
37.207100	1438.907205	17.435213
37.566675	1435.088738	17.440231
37.384447	1441.665062	17.445248
37.500683	1438.797004	17.450266
37.667928	1437.356244	17.455283
37.404913	1456.874590	17.460301
38.075927	1462.081541	17.465319
37.893529	1468.915103	17.470336
38.004316	1464.462244	17.475354
38.077716	1456.390973	17.480371
37.679510	1458.127567	17.485389
38.387188	1454.520997	17.490407
37.707141	1446.664288	17.495424
37.769766	1445.078186	17.500442
37.851418	1462.631850	17.505459
37.780478	1469.089760	17.510477
38.231015	1457.825546	17.515495
38.197822	1467.357525	17.520512
38.278436	1471.724236	17.525530
38.366741	1469.358507	17.530547
38.115515	1474.701544	17.535565
38.297493	1462.010117	17.540583
38.562423	1468.765254	17.545600
38.442022	1455.457434	17.550618
38.652456	1462.377781	17.555635
38.572344	1474.121919	17.560653
38.540051	1463.840806	17.565671
38.389514	1470.367256	17.570688
38.446460	1465.087677	17.575706
38.531962	1458.358673	17.580723
38.501827	1463.257442	17.585741
38.627382	1467.179668	17.590759
38.674546	1465.651874	17.595776
38.340515	1461.164565	17.600794
38.541322	1465.451541	17.605811
38.492070	1467.336193	17.610829
38.406687	1463.698016	17.615847
38.827600	1475.182913	17.620864
38.672635	1497.027184	17.625882
39.100420	1489.491638	17.630899
38.980468	1501.332606	17.635917
39.145578	1490.830431	17.640935
39.153140	1498.878805	17.645952
39.370859	1492.302523	17.650970
39.504103	1489.495452	17.655987
38.937092	1478.862295	17.661005
39.080220	1480.757952	17.666023
39.334904	1488.280823	17.671040
38.795208	1500.219411	17.676058
39.545013	1488.141351	17.681075
39.383979	1500.730579	17.686093
39.301700	1494.848681	17.691111
39.377919	1502.186084	17.696128
38.887792	1494.367486	17.701146
39.421276	1492.725157	17.706163
39.448976	1491.169790	17.711181
39.409061	1489.978365	17.716199
39.632034	1486.511232	17.721216
39.262293	1499.227345	17.726234
39.352820	1491.036129	17.731251
39.271886	1501.565214	17.736269
39.448281	1519.473510	17.741287
39.743494	1520.937486	17.746304
39.674683	1521.708373	17.751322
39.786838	1518.875558	17.756339
40.078818	1521.548966	17.761357
40.109979	1515.979315	17.766375
39.928144	1512.117400	17.771392
39.700178	1520.342570	17.776410
39.972628	1519.397848	17.781427
40.045992	1519.991896	17.786445
39.968314	1513.288106	17.791463
39.816160	1517.341945	17.796480
39.949688	1515.333951	17.801498
40.358656	1521.555673	17.806515
40.248375	1528.581476	17.811533
40.438694	1527.855141	17.816551
40.515837	1519.033663	17.821568
40.203810	1521.787676	17.826586
40.266346	1535.099503	17.831603
40.520886	1541.612503	17.836621
40.734808	1546.942728	17.841639
40.623642	1543.010543	17.846656
40.416175	1547.232880	17.851674
40.609653	1544.180229	17.856691
40.326497	1549.927950	17.861709
40.546195	1541.586324	17.866727
40.958113	1538.420965	17.871744
40.532013	1544.278790	17.876762
40.914393	1536.670235	17.881779
40.899314	1544.584600	17.886797
40.779511	1540.207823	17.891815
40.930626	1538.614676	17.896832
40.782849	1538.494420	17.901850
40.824080	1531.197478	17.906867
40.884839	1538.590851	17.911885
40.797430	1536.791919	17.916903
41.247340	1530.181733	17.921920
40.762812	1533.549237	17.926938
41.238515	1538.286339	17.931955
41.188830	1542.057202	17.936973
40.885823	1539.751514	17.941991
41.009529	1545.247931	17.947008
41.108621	1568.359025	17.952026
41.589065	1562.226894	17.957043
41.280459	1574.553419	17.962061
41.729690	1562.825272	17.967079
41.863419	1571.585837	17.972096
41.571108	1570.292296	17.977114
41.534379	1571.650338	17.982131
41.335589	1568.874973	17.987149
41.515131	1564.799670	17.992167
41.655430	1564.834823	17.997184
41.666129	1570.591529	18.002202
41.776855	1565.006023	18.007219
41.540203	1570.397896	18.012237
41.483639	1571.060648	18.017255
42.068538	1557.949355	18.022272
41.966967	1571.456497	18.027290
41.865428	1561.545810	18.032307
41.813857	1565.712612	18.037325
41.837686	1563.873912	18.042343
41.767641	1564.051943	18.047360
42.087671	1578.350756	18.052378
42.235612	1581.568629	18.057395
42.378151	1580.671367	18.062413
42.766073	1575.742458	18.067431
42.501035	1556.493235	18.072448
42.284046	1559.148723	18.077466
42.247479	1560.262123	18.082483
42.325916	1553.171604	18.087501
42.416314	1553.788106	18.092519
42.636955	1553.863143	18.097536
42.281773	1564.188252	18.102554
42.756224	1567.141679	18.107571
43.061286	1572.141973	18.112589
42.385619	1567.451132	18.117607
42.560467	1552.040889	18.122624
42.765712	1566.832285	18.127642
42.726471	1575.687297	18.132659
42.613649	1575.490675	18.137677
42.836267	1575.028972	18.142695
43.203479	1576.882610	18.147712
43.046976	1576.449125	18.152730
42.917102	1575.029785	18.157747
43.233595	1570.091034	18.162765
43.047169	1576.867871	18.167783
42.789536	1553.777552	18.172800
42.943151	1565.618986	18.177818
43.045285	1582.892664	18.182835
43.008112	1584.924062	18.187853
42.942152	1578.912893	18.192871
43.146422	1580.422842	18.197888
42.801819	1583.326000	18.202906
43.109999	1582.373217	18.207923
43.494495	1571.569355	18.212941
43.299772	1573.697455	18.217959
43.626405	1569.387110	18.222976
43.410233	1570.802087	18.227994
43.537312	1571.192508	18.233011
43.646269	1568.289404	18.238029
43.583365	1576.096579	18.243047
43.595399	1568.760229	18.248064
43.849540	1583.268552	18.253082
44.028212	1594.045748	18.258099
44.194902	1578.698915	18.263117
43.540714	1574.666131	18.268135
43.760593	1566.056249	18.273152
43.852825	1576.195959	18.278170
43.751081	1594.881771	18.283187
44.108998	1593.603289	18.288205
43.955301	1593.837922	18.293223
44.257516	1598.236184	18.298240
43.939591	1601.304985	18.303258
43.833637	1598.079846	18.308275
44.244886	1600.864028	18.313293
44.165546	1604.054446	18.318311
44.388930	1597.515753	18.323328
44.428357	1597.874534	18.328346
44.275407	1601.896275	18.333363
44.221254	1602.594039	18.338381
43.926347	1599.076552	18.343399
44.243084	1601.151397	18.348416
44.260243	1615.570129	18.353434
44.401099	1615.996107	18.358451
44.396503	1627.707088	18.363469
44.521543	1633.646153	18.368487
44.523345	1630.743610	18.373504
44.660311	1630.913794	18.378522
44.528617	1635.938937	18.383539
44.651600	1636.386643	18.388557
44.516990	1632.299290	18.393575
44.875529	1639.920513	18.398592
44.802177	1659.868225	18.403610
44.971933	1658.326365	18.408627
45.195108	1660.717390	18.413645
45.028527	1665.710352	18.418663
45.086957	1659.416603	18.423680
45.380762	1660.572490	18.428698
45.578693	1660.622834	18.433715
45.500530	1659.568849	18.438733
45.173959	1668.352548	18.443751
45.352748	1661.735993	18.448768
45.614077	1653.058885	18.453786
45.558232	1653.859173	18.458803
45.755217	1628.283090	18.463821
45.426361	1633.148546	18.468839
45.292773	1629.971854	18.473856
45.349579	1650.738043	18.478874
45.591687	1650.273229	18.483891
45.411786	1656.998724	18.488909
45.413548	1663.996496	18.493927
45.473617	1657.679676	18.498944
45.319031	1664.178542	18.503962
45.472249	1658.174857	18.508979
45.933768	1659.830198	18.513997
46.122473	1675.090767	18.519015
45.834071	1682.620130	18.524032
46.346035	1685.333993	18.529050
46.255824	1681.624955	18.534067
46.026754	1665.676515	18.539085
46.032060	1668.534106	18.544103
46.119856	1668.176492	18.549120
46.275232	1679.816381	18.554138
46.055756	1677.620836	18.559155
46.724104	1669.713333	18.564173
46.418024	1672.046407	18.569191
46.395369	1665.608277	18.574208
46.840928	1663.159581	18.579226
46.576356	1672.710507	18.584243
46.877759	1674.658815	18.589261
47.008991	1676.141096	18.594279
46.847461	1646.418044	18.599296
46.790515	1642.735959	18.604314
46.390704	1645.634562	18.609331
46.997730	1650.690548	18.614349
46.795312	1657.088496	18.619367
46.876617	1657.957363	18.624384
47.080936	1652.021825	18.629402
46.994715	1663.175605	18.634419
47.269216	1662.836192	18.639437
46.715683	1655.102341	18.644455
46.973042	1653.673930	18.649472
46.929312	1663.177042	18.654490
47.022774	1665.307172	18.659507
47.508012	1664.241984	18.664525
47.371615	1665.318614	18.669543
47.342512	1671.110811	18.674560
47.413191	1669.629585	18.679578
47.411005	1659.238133	18.684595
47.462123	1661.564574	18.689613
47.321279	1668.147771	18.694631
47.419207	1670.890699	18.699648
47.618445	1666.506259	18.704666
47.347676	1660.843914	18.709683
47.607374	1660.793954	18.714701
47.422494	1671.368056	18.719719
47.176425	1667.642979	18.724736
47.419095	1672.482578	18.729754
47.411493	1693.666533	18.734771
47.688648	1697.917805	18.739789
47.917091	1702.172914	18.744807
47.758427	1698.856268	18.749824
47.965569	1696.027147	18.754842
47.792792	1705.483225	18.759859
47.918379	1700.758932	18.764877
47.753706	1699.166581	18.769895
47.808588	1716.700438	18.774912
48.118713	1717.738891	18.779930
48.103603	1737.999908	18.784947
48.312661	1731.036342	18.789965
48.329900	1736.725215	18.794983
48.493766	1736.734586	18.800000
48.654705	1723.958192	18.805018
48.574332	1732.399840	18.810035
48.485472	1724.181258	18.815053
48.690471	1731.979610	18.820071
48.639399	1721.857046	18.825088
48.705600	1728.391517	18.830106
48.585914	1720.136167	18.835123
48.659201	1719.625128	18.840141
48.680329	1730.489689	18.845159
49.007291	1722.011297	18.850176
48.842007	1718.881328	18.855194
48.821046	1734.478222	18.860211
49.045015	1740.595045	18.865229
49.238819	1751.827720	18.870247
49.274946	1757.187167	18.875264
49.447418	1746.619924	18.880282
49.076503	1737.704598	18.885299
49.513353	1733.703834	18.890317
49.444136	1735.082804	18.895335
49.235332	1733.930879	18.900352
49.516868	1737.698520	18.905370
49.274641	1749.056581	18.910387
49.077526	1749.875472	18.915405
49.315553	1750.684741	18.920423
49.342221	1749.466943	18.925440
49.898480	1747.819383	18.930458
49.561505	1763.741219	18.935475
49.539578	1752.508874	18.940493
49.710466	1749.261571	18.945511
49.529638	1762.302517	18.950528
49.977951	1743.396262	18.955546
49.736990	1746.685638	18.960563
49.812027	1757.053957	18.965581
50.243170	1774.003241	18.970599
50.112748	1772.173385	18.975616
50.161418	1775.750074	18.980634
50.187142	1769.813084	18.985651
50.102961	1764.341962	18.990669
50.052835	1772.465759	18.995687
50.091562	1778.807209	19.000704
50.539346	1761.935051	19.005722
50.565333	1770.358971	19.010739
50.549105	1766.483160	19.015757
50.631128	1771.187169	19.020775
50.365860	1768.250898	19.025792
50.551949	1756.733675	19.030810
50.602873	1769.195728	19.035827
50.264612	1769.842853	19.040845
50.386436	1769.593860	19.045863
50.516137	1768.479971	19.050880
50.714926	1768.472761	19.055898
50.451693	1772.292687	19.060915
50.699310	1788.096929	19.065933
50.954139	1797.893091	19.070951
50.949308	1797.659578	19.075968
51.119304	1799.456605	19.080986
51.066797	1801.345752	19.086003
51.222603	1807.422348	19.091021
51.141463	1799.804210	19.096039
50.860047	1805.342528	19.101056
51.440448	1800.338800	19.106074
51.256130	1802.672925	19.111091
51.213213	1797.413086	19.116109
51.273720	1796.587100	19.121127
51.339239	1800.467079	19.126144
51.002856	1798.264990	19.131162
51.052658	1821.036689	19.136179
51.674253	1826.192667	19.141197
51.586902	1823.063618	19.146215
51.532714	1831.189668	19.151232
51.508379	1826.066863	19.156250
51.830039	1820.709542	19.161267
52.038037	1823.972951	19.166285
51.872102	1816.904761	19.171303
51.782341	1821.117055	19.176320
51.932589	1835.616245	19.181338
52.399322	1844.165766	19.186355
52.298337	1839.551501	19.191373
52.231129	1834.194057	19.196391
52.117267	1840.481214	19.201408
52.537091	1845.071593	19.206426
52.808889	1845.154205	19.211443
52.468648	1830.341804	19.216461
52.573683	1821.091739	19.221479
52.184862	1815.921670	19.226496
52.359777	1822.568627	19.231514
52.267666	1837.722349	19.236531
52.574762	1843.365820	19.241549
52.862648	1827.681625	19.246567
52.746182	1850.215604	19.251584
52.686102	1842.666448	19.256602
53.011758	1850.941154	19.261619
52.610235	1844.105591	19.266637
53.011922	1845.426771	19.271655
52.662135	1848.765775	19.276672
52.713619	1839.469966	19.281690
52.550443	1850.361652	19.286707
52.760636	1857.680228	19.291725
53.230982	1860.760222	19.296743
52.991866	1879.695625	19.301760
53.458843	1868.199587	19.306778
53.428198	1877.556024	19.311795
53.393759	1875.440269	19.316813
53.481409	1877.771144	19.321831
53.448883	1878.906733	19.326848
53.398104	1878.177147	19.331866
53.264560	1868.772395	19.336883
53.470268	1871.818302	19.341901
53.622574	1872.131558	19.346919
53.420979	1878.497221	19.351936
53.555878	1871.973306	19.356954
53.666893	1886.876018	19.361971
53.551125	1905.889316	19.366989
54.242804	1897.130843	19.372007
54.245837	1907.122191	19.377024
54.013864	1905.392676	19.382042
54.150988	1904.108483	19.387059
54.065726	1907.652292	19.392077
54.204681	1898.672851	19.397095
54.110339	1902.443851	19.402112
54.256368	1903.658724	19.407130
54.137862	1898.527316	19.412147
54.222086	1897.440335	19.417165
54.259376	1899.811494	19.422183
53.960935	1908.993571	19.427200
53.967378	1919.969162	19.432218
54.605389	1932.254345	19.437235
54.898432	1930.906740	19.442253
55.226250	1918.691913	19.447271
55.151824	1929.188806	19.452288
55.405959	1916.678971	19.457306
55.148254	1898.579654	19.462323
54.975676	1896.650320	19.467341
55.042461	1883.852621	19.472359
55.060417	1881.074875	19.477376
55.175716	1890.718737	19.482394
55.278302	1892.563496	19.487411
55.191538	1894.692514	19.492429
55.460568	1897.746419	19.497447
55.473138	1894.519615	19.502464
55.181342	1887.480116	19.507482
55.276717	1891.639307	19.512499
55.192416	1908.486900	19.517517
55.335539	1910.416437	19.522535
55.265639	1920.204694	19.527552
55.535108	1912.753962	19.532570
55.368531	1918.952026	19.537587
55.381728	1927.076036	19.542605
55.458458	1911.511951	19.547623
55.509950	1926.807254	19.552640
55.723463	1938.943840	19.557658
55.875306	1947.343857	19.562675
55.650722	1949.174731	19.567693
55.830265	1941.435499	19.572711
55.880900	1945.728478	19.577728
55.741344	1947.887947	19.582746
56.166126	1942.523574	19.587763
55.867699	1952.909908	19.592781
55.993136	1965.644983	19.597799
55.999203	1963.660404	19.602816
56.166359	1974.690635	19.607834
56.292910	1970.977627	19.612851
56.042210	1977.934012	19.617869
56.365284	1980.293428	19.622887
56.533922	1981.698197	19.627904
56.632972	1998.742397	19.632922
56.925694	1999.116637	19.637939
56.834706	2013.795275	19.642957
57.118814	1997.699339	19.647975
57.113472	1995.779500	19.652992
56.918588	1985.818912	19.658010
56.813915	1986.789038	19.663027
57.104260	2005.526895	19.668045
56.944568	2000.059862	19.673063
57.154052	2002.313906	19.678080
57.105630	1991.860373	19.683098
57.396322	1997.772382	19.688115
57.234450	1995.608502	19.693133
57.574236	1987.411076	19.698151
57.536124	1998.239665	19.703168
57.570299	2000.410762	19.708186
57.618405	1991.315971	19.713203
57.722891	1997.664332	19.718221
57.742549	1998.459676	19.723239
57.749625	1988.794875	19.728256
57.589977	1989.411947	19.733274
57.736519	1980.013579	19.738291
57.538272	1993.598669	19.743309
57.676704	1992.798785	19.748327
58.115651	2010.266237	19.753344
57.857443	2023.672141	19.758362
58.357531	2018.619011	19.763379
58.281579	2027.735001	19.768397
58.220456	2016.842996	19.773415
58.451313	2021.158381	19.778432
58.887454	2015.818127	19.783450
59.061077	1997.374596	19.788467
58.754666	1994.013800	19.793485
58.856664	1978.302458	19.798503
58.951125	1971.549764	19.803520
58.429950	1974.990067	19.808538
58.655757	1977.118013	19.813555
58.397029	1975.319606	19.818573
58.496520	1980.627342	19.823591
58.768979	1980.956832	19.828608
58.522014	1978.557184	19.833626
58.906712	1973.662481	19.838643
58.616968	1997.946121	19.843661
59.099059	1996.791745	19.848679
59.120389	2007.354439	19.853696
58.869417	2004.875195	19.858714
58.940749	1999.953378	19.863731
58.809861	2006.196914	19.868749
58.893441	2006.088520	19.873767
58.969501	2011.224599	19.878784
59.045489	2027.541788	19.883802
59.439187	2025.004559	19.888819
59.436830	2040.705001	19.893837
59.646398	2035.455149	19.898855
59.609179	2027.707967	19.903872
59.613808	2037.743198	19.908890
59.676282	2036.401681	19.913907
59.699257	2034.631489	19.918925
59.423441	2041.499881	19.923943
59.675767	2052.654238	19.928960
59.638943	2062.760596	19.933978
59.976738	2062.509404	19.938995
60.123631	2066.114547	19.944013
60.000481	2063.092622	19.949031
60.503287	2062.543746	19.954048
60.368090	2067.932204	19.959066
60.653484	2059.740267	19.964083
60.298798	2054.482077	19.969101
60.326182	2054.642215	19.974119
60.457333	2057.497117	19.979136
60.561040	2057.648228	19.984154
60.603539	2061.970069	19.989171
60.844747	2083.824399	19.994189
60.888276	2084.124332	19.999207
60.845834	2083.060685	20.004224
60.993047	2083.722424	20.009242
60.824956	2074.982196	20.014259
61.226010	2080.991477	20.019277
60.780680	2085.135491	20.024295
60.874234	2083.449212	20.029312
61.252006	2087.828496	20.034330
61.224778	2079.705285	20.039347
61.157995	2088.457240	20.044365
60.974985	2086.330540	20.049383
61.326677	2079.790048	20.054400
61.029680	2086.762521	20.059418
61.671701	2102.864454	20.064435
61.688931	2111.028825	20.069453
61.968139	2119.594260	20.074471
62.067540	2121.351459	20.079488
61.683796	2107.218235	20.084506
61.797443	2104.612390	20.089523
61.721335	2109.041257	20.094541
61.590289	2116.749468	20.099559
61.930937	2109.723834	20.104576
61.942537	2114.116691	20.109594
61.880933	2117.482158	20.114611
61.747783	2124.688087	20.119629
61.968128	2109.266854	20.124647
62.033315	2112.427253	20.129664
61.901171	2126.720853	20.134682
62.441972	2136.272633	20.139699
62.351961	2137.163346	20.144717
62.300294	2148.844497	20.149735
62.552911	2139.884537	20.154752
62.368583	2140.982218	20.159770
62.503494	2143.064119	20.164787
62.815625	2148.494531	20.169805
62.534021	2145.670121	20.174823
62.838694	2141.488967	20.179840
62.821075	2164.319936	20.184858
63.171747	2147.030994	20.189875
63.498150	2148.062952	20.194893
63.204233	2157.742365	20.199911
63.569468	2147.913363	20.204928
63.106251	2143.472398	20.209946
63.250960	2144.241514	20.214963
63.447535	2150.075779	20.219981
63.360887	2155.712164	20.224999
63.577976	2156.298263	20.230016
63.408316	2162.232631	20.235034
63.614653	2154.507892	20.240051
63.620719	2156.215482	20.245069
63.950268	2151.251645	20.250087
63.849458	2150.049426	20.255104
63.616086	2155.334014	20.260122
63.540211	2152.027656	20.265139
63.576199	2155.144740	20.270157
63.945424	2166.336388	20.275175
64.299859	2180.254325	20.280192
64.019798	2184.929693	20.285210
64.043045	2183.977482	20.290227
64.212791	2181.258061	20.295245
64.095200	2187.029179	20.300263
64.206559	2181.742237	20.305280
64.052331	2183.977233	20.310298
64.178097	2177.774776	20.315315
64.391685	2192.279165	20.320333
64.538081	2212.637790	20.325351
64.867066	2208.531397	20.330368
64.726745	2215.526924	20.335386
64.823272	2205.650282	20.340403
64.986562	2209.023164	20.345421
64.713371	2213.127174	20.350439
65.149222	2207.027061	20.355456
64.805108	2209.105138	20.360474
64.991407	2208.369975	20.365491
64.952372	2208.292934	20.370509
64.938979	2224.721348	20.375527
65.352129	2239.484992	20.380544
65.336550	2242.003077	20.385562
65.395824	2247.974907	20.390579
65.600504	2245.225519	20.395597
65.268742	2251.959773	20.400615
65.719853	2247.344639	20.405632
65.327503	2242.543098	20.410650
65.804767	2241.358013	20.415667
65.843209	2245.678195	20.420685
65.542437	2248.513923	20.425703
65.903139	2255.403607	20.430720
65.944743	2268.465377	20.435738
65.849062	2266.871397	20.440755
66.325738	2269.042756	20.445773
66.397679	2269.354680	20.450791
66.510367	2262.056989	20.455808
66.432042	2268.610820	20.460826
66.651179	2263.641744	20.465843
66.711126	2268.594063	20.470861
66.608167	2268.185840	20.475879
66.727306	2259.724551	20.480896
66.314774	2260.894031	20.485914
66.718100	2262.255893	20.490931
66.825033	2256.296315	20.495949
66.876691	2266.428032	20.500967
67.149099	2266.860582	20.505984
66.830613	2263.314440	20.511002
66.518789	2264.437968	20.516019
66.693262	2266.864395	20.521037
66.672843	2291.476834	20.526055
67.235881	2290.740578	20.531072
66.926042	2295.006985	20.536090
67.343896	2286.660864	20.541107
67.854672	2282.689854	20.546125
67.433885	2285.289090	20.551143
67.799232	2286.380134	20.556160
67.705736	2282.703715	20.561178
67.746111	2276.713841	20.566195
67.625643	2275.768813	20.571213
67.833539	2280.452913	20.576231
68.166924	2284.455484	20.581248
67.888583	2284.051633	20.586266
67.776311	2303.902604	20.591283
68.325096	2298.934431	20.596301
68.047433	2319.645580	20.601319
68.325755	2311.121118	20.606336
68.745561	2309.665953	20.611354
68.642531	2313.052230	20.616371
68.581635	2301.807585	20.621389
68.464824	2307.621888	20.626407
68.645175	2306.065687	20.631424
68.604224	2307.659659	20.636442
68.682736	2305.398401	20.641459
68.872113	2301.237949	20.646477
68.581773	2310.400105	20.651495
69.140638	2302.466469	20.656512
69.052552	2305.353238	20.661530
68.616983	2311.891697	20.666547
68.724102	2304.423398	20.671565
68.707722	2306.923530	20.676583
68.778561	2306.446685	20.681600
68.996624	2325.255477	20.686618
68.967678	2327.111830	20.691635
69.420413	2323.745513	20.696653
68.943068	2341.909322	20.701671
69.263741	2340.572221	20.706688
69.409253	2337.674935	20.711706
69.234141	2345.707289	20.716723
69.803801	2354.637140	20.721741
69.802854	2366.971111	20.726759
69.929771	2365.182730	20.731776
69.705688	2358.837771	20.736794
69.517045	2370.147651	20.741811
69.815808	2354.030895	20.746829
69.964079	2367.867837	20.751847
70.200953	2369.249964	20.756864
70.487629	2384.980980	20.761882
70.469164	2389.411752	20.766899
70.281421	2387.054504	20.771917
70.507745	2384.738983	20.776935
70.742791	2379.049961	20.781952
70.811353	2382.025032	20.786970
70.646676	2375.474731	20.791987
71.030294	2375.959555	20.797005
70.911445	2377.477860	20.802023
71.185615	2383.863830	20.807040
71.528748	2373.110027	20.812058
70.832501	2376.007277	20.817075
71.108705	2367.009594	20.822093
70.865168	2376.604030	20.827111
71.142576	2375.624645	20.832128
71.388558	2366.900009	20.837146
71.143525	2372.608933	20.842163
71.674282	2374.063753	20.847181
71.464632	2372.910337	20.852199
71.492794	2396.498933	20.857216
71.857216	2396.547902	20.862234
71.869157	2404.117044	20.867251
72.014104	2398.389683	20.872269
71.776015	2400.957441	20.877287
71.871869	2399.487859	20.882304
71.985239	2410.848715	20.887322
71.989670	2415.033572	20.892339
72.450064	2403.767853	20.897357
72.271719	2401.931400	20.902375
71.986937	2400.200020	20.907392
71.708176	2394.268860	20.912410
71.919901	2403.003331	20.917427
72.343387	2413.213503	20.922445
72.209549	2427.598125	20.927463
72.786495	2434.119106	20.932480
72.833999	2429.634358	20.937498
72.592949	2434.224922	20.942515
72.736954	2427.465690	20.947533
72.830500	2427.033202	20.952551
72.906207	2432.717741	20.957568
73.104071	2424.318529	20.962586
73.151527	2427.288323	20.967603
73.176532	2422.445332	20.972621
73.105714	2425.000576	20.977639
73.203717	2428.888127	20.982656
73.277808	2439.481263	20.987674
73.236313	2459.119789	20.992691
73.222932	2453.386193	20.997709
73.572610	2461.018704	21.002727
73.552068	2459.982214	21.007744
74.003109	2453.054442	21.012762
73.539360	2465.356901	21.017779
73.956392	2455.827778	21.022797
74.048380	2458.987912	21.027815
73.828464	2457.390127	21.032832
74.099682	2469.489637	21.037850
74.383639	2485.663262	21.042867
74.253733	2479.323683	21.047885
74.252425	2489.744030	21.052903
74.314449	2491.556005	21.057920
74.631706	2486.801679	21.062938
74.345721	2481.965789	21.067955
74.643793	2487.824907	21.072973
74.725634	2479.295500	21.077991
74.684824	2475.752217	21.083008
75.124802	2459.756772	21.088026
74.726995	2481.634164	21.093043
74.786762	2477.023163	21.098061
74.898350	2475.094053	21.103079
75.114312	2489.719496	21.108096
75.254269	2497.707978	21.113114
75.444890	2497.829502	21.118131
75.671845	2495.800184	21.123149
75.624010	2511.511532	21.128167
75.517270	2503.288282	21.133184
75.774668	2494.502755	21.138202
75.365575	2518.715046	21.143219
75.564796	2507.036247	21.148237
75.630106	2496.487914	21.153255
75.640944	2503.268328	21.158272
75.822580	2497.318763	21.163290
75.323425	2495.592455	21.168307
75.733977	2522.954141	21.173325
75.901136	2527.868212	21.178343
75.790856	2536.080687	21.183360
76.195690	2526.587288	21.188378
76.329695	2542.366421	21.193395
76.344358	2538.430415	21.198413
76.240522	2535.648371	21.203431
76.242438	2543.644734	21.208448
76.546774	2552.322835	21.213466
76.675759	2559.715286	21.218483
76.852762	2558.326352	21.223501
76.925229	2554.160089	21.228519
76.898930	2550.772580	21.233536
76.977140	2542.825012	21.238554
76.842678	2550.766042	21.243571
76.617717	2559.266622	21.248589
77.154244	2566.774213	21.253607
77.007450	2579.867094	21.258624
77.252981	2577.992910	21.263642
77.401321	2591.738808	21.268659
77.475401	2582.667824	21.273677
77.412245	2582.222566	21.278695
77.460173	2580.787353	21.283712
77.833629	2580.705881	21.288730
77.693812	2584.456777	21.293747
77.429980	2596.486762	21.298765
77.993565	2607.293785	21.303783
77.937747	2615.415025	21.308800
77.680147	2608.158124	21.313818
77.919368	2609.696435	21.318835
77.975777	2621.248243	21.323853
78.203531	2630.319320	21.328871
78.131944	2643.877733	21.333888
78.516478	2633.165907	21.338906
78.522519	2645.985120	21.343923
78.781786	2655.291888	21.348941
78.590278	2645.088034	21.353959
78.740072	2640.638037	21.358976
78.698497	2634.561187	21.363994
78.858327	2662.887379	21.369011
78.890223	2669.750252	21.374029
79.187972	2666.274067	21.379047
78.865103	2670.555245	21.384064
79.305813	2668.234595	21.389082
79.277976	2675.790557	21.394099
79.045674	2674.491273	21.399117
79.322985	2672.454687	21.404135
79.287645	2698.759034	21.409152
79.740632	2696.294833	21.414170
79.655250	2706.147440	21.419187
79.910796	2703.871260	21.424205
79.779238	2698.796712	21.429223
79.767602	2705.179634	21.434240
80.093628	2694.540810	21.439258
80.012037	2701.110301	21.444275
80.081101	2703.331788	21.449293
80.463123	2717.351247	21.454311
80.338061	2730.729482	21.459328
80.710488	2723.607244	21.464346
80.841152	2726.001404	21.469363
80.592958	2732.782331	21.474381
80.903231	2716.487929	21.479399
80.644965	2728.687042	21.484416
80.818777	2723.529962	21.489434
80.660188	2721.268695	21.494451
80.702017	2720.463728	21.499469
80.936013	2720.085134	21.504487
80.628188	2722.481575	21.509504
80.608894	2725.704350	21.514522
81.050327	2753.055250	21.519539
81.123571	2760.016977	21.524557
81.194219	2763.531408	21.529575
81.278116	2755.582818	21.534592
81.128530	2750.753403	21.539610
81.587060	2769.426880	21.544627
81.395414	2786.493976	21.549645
81.763967	2779.094654	21.554663
82.021649	2779.738809	21.559680
81.880309	2782.100843	21.564698
82.018534	2784.112301	21.569715
81.560452	2789.016833	21.574733
82.051370	2795.530461	21.579751
81.991117	2812.829135	21.584768
82.062697	2811.240672	21.589786
82.103269	2817.262915	21.594803
82.127934	2828.931650	21.599821
82.682844	2839.379174	21.604839
82.479013	2849.068272	21.609856
82.803300	2842.304484	21.614874
83.170497	2841.887339	21.619891
82.954908	2844.782749	21.624909
83.537740	2835.075911	21.629927
83.515848	2844.695874	21.634944
83.154398	2840.977879	21.639962
83.332651	2837.708712	21.644979
83.346441	2842.479013	21.649997
83.410243	2836.681828	21.655015
83.349463	2841.244556	21.660032
83.392447	2836.230225	21.665050
83.353901	2857.549810	21.670067
83.297844	2875.872062	21.675085
83.991961	2866.112060	21.680103
83.959580	2869.477758	21.685120
83.710885	2878.240317	21.690138
83.962234	2867.570800	21.695155
84.042218	2879.086802	21.700173
84.416331	2887.882195	21.705191
84.473910	2897.664934	21.710208
84.350347	2894.003382	21.715226
84.765418	2894.878093	21.720243
84.733388	2890.328799	21.725261
84.648672	2886.864787	21.730279
84.300346	2894.017307	21.735296
84.439101	2895.230279	21.740314
84.714058	2895.546025	21.745331
84.689382	2908.154047	21.750349
84.905473	2918.917606	21.755367
85.035636	2923.307530	21.760384
85.227603	2926.332255	21.765402
85.362380	2923.729976	21.770419
85.342293	2926.923030	21.775437
85.485408	2916.610558	21.780455
85.459144	2927.932729	21.785472
85.338869	2930.360649	21.790490
85.897545	2927.741111	21.795507
85.710545	2943.910116	21.800525
85.554599	2951.170429	21.805543
85.720072	2951.274730	21.810560
85.759138	2952.198397	21.815578
86.054484	2948.694211	21.820595
85.925587	2959.264246	21.825613
86.347007	2970.211418	21.830631
86.253510	2978.820281	21.835648
86.457833	2990.194615	21.840666
86.564596	2983.286102	21.845683
86.367092	2987.071472	21.850701
86.925844	2986.802339	21.855719
86.637493	2986.740668	21.860736
87.166519	2979.837973	21.865754
87.180888	2975.118422	21.870771
86.895085	2983.498370	21.875789
87.393953	2974.305910	21.880807
87.245112	2985.562718	21.885824
87.216816	2996.271700	21.890842
87.307105	2998.329377	21.895859
87.449817	3003.394607	21.900877
87.804190	3006.432780	21.905895
87.478308	3001.712419	21.910912
87.600131	3006.438800	21.915930
87.413792	2999.455883	21.920947
87.858235	3011.209637	21.925965
88.125290	3021.048727	21.930983
88.310894	3033.720077	21.936000
88.152867	3028.132823	21.941018
88.460956	3028.706809	21.946035
88.564282	3031.931335	21.951053
88.628668	3033.864928	21.956071
88.608946	3036.504164	21.961088
88.410437	3034.424632	21.966106
88.873719	3021.330653	21.971123
88.469124	3027.593886	21.976141
88.648236	3018.113358	21.981159
88.594397	3029.381007	21.986176
88.524059	3052.113216	21.991194
89.025620	3056.075024	21.996211
89.052470	3060.744986	22.001229
88.795121	3059.227045	22.006247
88.799248	3072.488234	22.011264
88.913382	3082.713601	22.016282
89.165577	3090.461894	22.021299
89.085414	3098.551099	22.026317
89.679331	3100.388454	22.031335
89.911640	3114.893137	22.036352
89.712885	3126.718092	22.041370
90.017101	3107.326477	22.046387
90.140409	3107.344681	22.051405
90.559936	3100.265096	22.056423
90.679533	3103.446139	22.061440
90.635758	3115.459547	22.066458
90.626820	3105.450444	22.071475
90.513366	3117.224031	22.076493
90.635046	3106.174627	22.081511
90.761602	3104.964386	22.086528
90.444638	3110.099027	22.091546
90.739623	3101.005866	22.096563
90.486683	3111.259115	22.101581
90.774628	3127.597222	22.106599
90.753111	3141.568956	22.111616
90.744454	3136.056956	22.116634
91.057260	3136.874836	22.121651
91.223588	3161.534475	22.126669
91.352712	3169.967926	22.131687
91.999624	3159.198932	22.136704
92.223470	3152.080518	22.141722
92.574192	3139.750898	22.146739
92.766032	3135.602406	22.151757
92.745681	3114.584658	22.156775
92.644675	3113.646696	22.161792
92.359971	3110.500070	22.166810
92.700463	3114.902135	22.171827
92.361738	3106.245135	22.176845
92.528117	3109.912722	22.181863
92.599196	3096.786828	22.186880
92.877190	3110.983730	22.191898
92.850267	3103.615063	22.196915
92.842523	3106.561547	22.201933
92.834617	3103.601262	22.206951
92.925858	3102.992918	22.211968
92.593773	3096.578330	22.216986
93.293835	3112.335459	22.222003
93.299532	3129.369909	22.227021
93.291656	3133.746512	22.232039
93.502242	3128.265628	22.237056
93.236564	3136.894175	22.242074
93.601068	3135.679025	22.247091
93.993464	3134.038579	22.252109
93.820982	3129.426653	22.257127
93.677496	3127.636464	22.262144
93.512173	3142.938512	22.267162
93.554705	3145.997341	22.272179
93.740438	3163.406661	22.277197
93.849548	3168.946926	22.282215
93.919362	3162.660942	22.287232
94.005947	3183.872943	22.292250
94.061559	3188.030194	22.297267
94.154111	3201.431578	22.302285
94.225500	3200.142812	22.307303
94.746956	3194.910462	22.312320
94.502991	3205.089187	22.317338
95.167082	3207.689415	22.322355
95.257696	3220.336744	22.327373
95.578452	3214.048478	22.332391
95.847502	3207.353904	22.337408
95.603241	3194.599157	22.342426
95.678984	3181.791029	22.347443
95.806414	3171.881275	22.352461
95.816133	3174.208268	22.357479
95.637081	3172.162584	22.362496
95.276235	3182.245871	22.367514
95.809928	3191.701945	22.372531
96.064830	3199.060481	22.377549
96.072958	3202.567682	22.382567
96.238288	3205.370163	22.387584
96.068253	3213.041902	22.392602
96.001270	3207.307118	22.397619
96.096317	3214.470110	22.402637
96.097515	3239.551105	22.407655
96.456037	3236.336486	22.412672
96.155554	3243.550769	22.417690
96.509020	3233.232062	22.422707
96.571868	3258.419680	22.427725
96.550210	3272.603954	22.432743
96.847781	3269.457259	22.437760
97.146832	3267.758529	22.442778
97.569919	3277.466715	22.447795
97.421171	3277.492121	22.452813
97.335577	3282.727585	22.457831
97.441402	3288.327417	22.462848
97.517111	3303.874385	22.467866
97.640787	3300.884424	22.472883
97.735537	3309.728557	22.477901
97.421452	3308.016683	22.482919
98.197075	3304.073971	22.487936
97.904526	3322.639022	22.492954
98.148928	3329.918275	22.497971
98.530449	3327.550328	22.502989
98.611866	3328.296563	22.508007
98.736077	3319.575838	22.513024
98.733063	3323.969029	22.518042
98.919695	3325.261720	22.523059
99.109939	3316.162319	22.528077
98.779794	3321.550858	22.533095
99.041918	3306.901266	22.538112
99.268915	3311.022568	22.543130
99.374659	3304.442883	22.548147
99.552534	3304.240782	22.553165
99.423337	3305.400550	22.558183
99.694174	3309.545539	22.563200
100.011275	3316.194106	22.568218
99.901117	3311.886052	22.573235
99.942045	3295.228843	22.578253
99.734351	3300.888117	22.583271
100.121304	3313.675490	22.588288
99.794546	3325.003409	22.593306
100.007960	3333.710638	22.598323
100.156691	3337.060147	22.603341
99.980249	3338.433552	22.608359
100.831488	3334.381231	22.613376
100.359916	3335.017418	22.618394
100.409975	3329.134913	22.623411
100.586345	3333.675708	22.628429
100.563569	3354.475891	22.633447
100.817036	3360.332252	22.638464
100.905794	3363.493884	22.643482
100.690801	3362.982350	22.648499
100.850582	3370.509537	22.653517
100.874552	3380.777025	22.658535
101.014345	3386.596459	22.663552
101.209544	3395.833681	22.668570
101.038313	3391.770549	22.673587
101.698755	3404.870738	22.678605
101.524556	3417.610026	22.683623
101.702796	3409.475335	22.688640
101.821397	3412.950024	22.693658
101.879134	3423.736849	22.698675
102.461296	3438.549494	22.703693
102.250393	3453.987357	22.708711
102.418755	3444.824501	22.713728
102.456746	3443.692862	22.718746
102.362190	3455.119154	22.723763
102.673251	3443.857580	22.728781
102.349530	3456.726943	22.733799
102.891460	3463.589879	22.738816
102.974478	3475.450418	22.743834
102.848338	3486.741749	22.748851
103.086691	3482.279736	22.753869
102.876127	3489.818844	22.758887
103.217546	3489.166656	22.763904
103.164963	3508.367833	22.768922
103.727173	3510.350326	22.773939
103.915808	3501.236907	22.778957
103.896419	3511.982605	22.783975
103.685628	3500.174886	22.788992
103.706024	3513.397694	22.794010
103.919758	3526.551923	22.799027
104.073088	3525.400312	22.804045
104.358985	3538.736560	22.809063
104.413786	3524.440768	22.814080
104.413451	3539.540708	22.819098
104.592824	3548.153589	22.824115
105.226508	3547.678988	22.829133
105.020565	3560.517073	22.834151
104.868256	3559.771339	22.839168
105.393693	3551.032120	22.844186
105.251307	3550.018129	22.849203
105.562599	3551.952537	22.854221
105.207570	3561.795225	22.859239
105.506145	3559.616680	22.864256
105.531758	3553.859915	22.869274
105.526511	3555.484514	22.874291
105.836412	3548.451305	22.879309
105.603070	3552.349517	22.884327
105.609822	3567.785830	22.889344
105.981184	3579.612272	22.894362
105.951384	3587.673262	22.899379
105.999812	3579.343635	22.904397
106.118610	3584.986352	22.909415
106.278726	3589.554992	22.914432
106.697346	3602.384768	22.919450
106.667702	3615.131067	22.924467
106.754095	3605.884424	22.929485
106.780795	3605.864544	22.934503
106.880062	3610.338269	22.939520
106.958941	3605.092969	22.944538
106.805965	3616.430370	22.949555
107.121439	3634.182997	22.954573
107.134621	3646.031211	22.959591
107.149470	3643.049096	22.964608
107.464771	3645.067836	22.969626
107.347315	3667.805366	22.974643
107.851877	3671.021903	22.979661
107.694687	3676.435696	22.984679
107.641598	3674.251067	22.989696
107.832616	3691.069392	22.994714
107.835964	3704.281717	22.999731
107.922353	3713.501091	23.004749
108.041237	3719.016407	23.009767
108.195342	3722.851306	23.014784
108.628175	3727.691951	23.019802
108.703502	3740.136061	23.024819
109.128057	3731.678716	23.029837
108.852881	3734.961397	23.034855
108.756410	3743.130649	23.039872
109.128028	3752.122058	23.044890
109.352114	3772.984947	23.049907
109.396344	3766.096266	23.054925
109.333422	3773.885734	23.059943
109.648289	3766.726550	23.064960
109.832390	3769.416801	23.069978
109.718233	3795.767938	23.074995
110.098112	3789.784667	23.080013
110.240541	3789.164987	23.085031
110.304190	3792.230810	23.090048
110.895485	3787.109838	23.095066
110.562240	3782.384887	23.100083
110.887143	3787.096445	23.105101
110.793083	3794.071183	23.110119
111.155842	3785.728288	23.115136
111.632451	3783.323868	23.120154
110.867297	3786.936428	23.125171
111.430145	3778.157284	23.130189
111.218358	3780.146029	23.135207
111.289258	3786.994553	23.140224
111.501451	3780.351268	23.145242
111.626202	3781.904815	23.150259
111.590508	3779.205278	23.155277
111.491625	3778.720052	23.160295
111.399899	3787.080519	23.165312
111.581637	3799.508497	23.170330
111.683481	3811.158627	23.175347
111.946296	3804.114712	23.180365
112.020570	3799.698436	23.185383
112.225433	3820.160112	23.190400
112.273341	3824.928439	23.195418
112.412928	3821.232556	23.200435
112.572506	3829.088838	23.205453
112.222070	3831.944582	23.210471
112.415638	3843.679230	23.215488
113.220056	3852.848699	23.220506
112.858287	3861.797432	23.225523
112.884804	3854.673961	23.230541
113.009728	3862.119639	23.235559
113.221663	3881.714937	23.240576
113.475848	3884.059699	23.245594
113.675969	3896.943457	23.250611
113.819659	3882.110794	23.255629
113.582952	3894.777861	23.260647
113.717081	3916.582784	23.265664
114.070079	3911.966267	23.270682
113.921680	3918.816782	23.275699
113.991980	3916.732802	23.280717
114.424170	3929.958759	23.285735
114.467204	3940.881257	23.290752
114.907254	3939.739747	23.295770
114.650624	3944.440248	23.300787
114.693601	3948.065579	23.305805
115.059235	3955.072503	23.310823
114.750476	3956.302648	23.315840
115.149985	3967.364203	23.320858
115.425394	3984.321236	23.325875
115.270362	3975.376395	23.330893
115.591098	3972.881948	23.335911
115.791634	3970.375201	23.340928
115.976035	3983.700507	23.345946
116.038058	4007.693796	23.350963
116.441149	4012.102675	23.355981
116.338072	4005.659818	23.360999
116.639686	4007.529751	23.366016
116.690092	4006.052312	23.371034
116.499900	4010.998696	23.376051
116.357992	4006.779674	23.381069
116.734024	4004.192229	23.386087
116.580478	4012.684617	23.391104
116.734600	4022.663542	23.396122
117.076267	4036.456279	23.401139
116.772099	4035.646627	23.406157
116.884958	4041.688527	23.411175
116.911960	4053.521493	23.416192
117.504847	4055.877567	23.421210
117.384252	4064.900459	23.426227
117.625107	4068.993020	23.431245
117.683691	4071.125133	23.436263
117.284106	4070.897104	23.441280
117.893211	4085.603844	23.446298
117.872138	4106.282096	23.451315
118.206805	4099.919651	23.456333
118.350684	4099.575852	23.461351
118.186271	4112.224497	23.466368
118.662524	4121.474002	23.471386
118.695584	4131.512427	23.476403
118.968209	4131.779018	23.481421
119.007347	4130.146027	23.486439
118.861376	4134.541803	23.491456
119.079917	4140.451248	23.496474
119.129178	4146.864421	23.501491
119.578909	4164.305995	23.506509
119.816852	4160.510955	23.511527
119.561792	4165.279717	23.516544
119.933512	4156.932825	23.521562
119.781635	4166.583821	23.526579
119.938154	4182.780437	23.531597
120.205168	4184.167378	23.536615
120.374153	4191.322991	23.541632
120.365174	4188.754429	23.546650
120.221947	4195.143249	23.551667
120.452405	4206.383773	23.556685
120.631541	4219.081569	23.561703
120.424344	4227.631410	23.566720
120.999506	4223.638616	23.571738
121.109579	4233.908704	23.576755
121.415684	4240.066195	23.581773
121.761833	4240.934682	23.586791
122.073351	4236.430883	23.591808
122.124683	4229.862610	23.596826
122.268998	4227.633833	23.601843
122.712122	4218.182810	23.606861
122.539468	4200.234638	23.611879
122.660102	4199.427252	23.616896
122.607281	4190.673667	23.621914
122.652531	4187.166593	23.626931
122.324421	4196.768617	23.631949
122.433277	4203.960572	23.636967
122.536714	4220.593651	23.641984
122.738865	4215.654953	23.647002
122.609392	4223.353788	23.652019
122.632422	4231.360291	23.657037
122.984549	4241.635841	23.662055
122.860915	4257.716728	23.667072
123.100294	4256.677998	23.672090
123.181287	4263.013786	23.677107
123.180453	4277.640189	23.682125
123.407110	4274.956154	23.687143
123.357664	4286.934449	23.692160
123.766822	4298.183523	23.697178
123.554858	4304.102681	23.702195
124.166488	4316.258007	23.707213
124.202188	4309.991134	23.712231
124.167077	4321.171824	23.717248
124.427147	4331.861757	23.722266
124.577439	4335.349707	23.727283
124.330015	4343.303420	23.732301
124.717746	4346.408938	23.737319
124.845830	4361.392481	23.742336
125.239561	4365.255421	23.747354
125.286550	4360.345350	23.752371
125.413903	4373.975905	23.757389
125.647866	4361.458561	23.762407
125.727225	4381.348649	23.767424
126.022046	4388.620392	23.772442
125.912365	4384.786323	23.777459
126.035991	4397.911649	23.782477
126.576095	4392.922149	23.787495
126.374127	4393.535049	23.792512
126.528960	4393.838523	23.797530
126.614406	4397.121273	23.802547
126.514400	4418.013158	23.807565
126.698634	4420.537516	23.812583
126.809375	4426.110253	23.817600
126.937333	4419.135540	23.822618
127.051449	4418.363010	23.827635
127.006739	4447.778658	23.832653
127.108611	4436.021025	23.837671
127.486000	4440.039211	23.842688
127.716893	4439.561952	23.847706
128.137282	4455.969323	23.852723
127.982838	4471.956232	23.857741
128.478587	4470.183523	23.862759
128.443104	4473.310138	23.867776
128.288264	4468.974253	23.872794
128.784499	4459.081923	23.877811
128.553440	4458.228332	23.882829
128.877469	4466.792727	23.887847
128.981469	4483.813072	23.892864
128.848343	4497.036856	23.897882
129.099590	4500.186986	23.902899
129.058862	4496.491366	23.907917
129.348804	4495.165278	23.912935
129.479566	4499.945788	23.917952
129.576089	4508.603127	23.922970
129.890780	4515.320285	23.927987
129.765253	4521.952662	23.933005
129.624169	4523.847627	23.938023
129.787920	4525.414703	23.943040
129.923168	4543.090179	23.948058
129.909562	4545.070238	23.953075
129.958178	4553.698267	23.958093
129.944577	4560.592881	23.963111
130.090799	4586.257239	23.968128
130.142428	4586.627524	23.973146
130.398088	4602.787552	23.978163
130.570070	4625.115372	23.983181
130.827131	4629.307780	23.988199
131.473649	4652.655860	23.993216
131.450998	4652.339392	23.998234
131.666880	4661.079274	24.003251
131.501044	4654.934862	24.008269
132.118612	4650.765267	24.013287
132.288463	4652.941086	24.018304
131.914187	4665.991849	24.023322
132.478871	4673.027171	24.028339
132.482316	4687.326813	24.033357
133.003712	4672.566869	24.038375
132.452662	4683.908775	24.043392
132.723950	4681.319824	24.048410
132.699171	4680.534027	24.053427
132.977152	4701.037194	24.058445
133.104087	4709.159556	24.063463
133.356021	4710.049391	24.068480
133.083902	4719.701040	24.073498
133.530962	4708.033691	24.078515
133.906643	4734.360321	24.083533
133.999391	4731.511106	24.088551
134.401921	4730.698078	24.093568
134.512534	4732.783443	24.098586
134.712299	4729.025028	24.103603
134.417924	4731.777594	24.108621
134.325043	4723.402983	24.113639
134.692978	4717.160058	24.118656
134.862839	4748.864474	24.123674
135.165501	4745.518409	24.128691
135.101616	4758.443449	24.133709
135.036035	4764.091633	24.138727
135.223649	4750.436676	24.143744
135.259397	4761.332624	24.148762
135.266556	4765.081875	24.153779
135.207331	4782.023171	24.158797
135.378418	4792.178500	24.163815
135.288248	4805.543614	24.168832
135.522897	4822.782680	24.173850
136.431167	4818.824730	24.178867
136.176674	4847.303026	24.183885
136.403879	4845.051500	24.188903
136.649605	4849.203296	24.193920
136.586539	4862.117281	24.198938
136.770322	4867.809134	24.203955
136.786921	4879.410766	24.208973
137.428365	4871.104645	24.213991
137.540235	4871.289106	24.219008
137.302445	4885.533786	24.224026
137.987808	4875.923353	24.229043
137.669103	4877.371503	24.234061
137.840554	4888.211290	24.239079
137.974276	4897.135920	24.244096
138.017028	4909.729398	24.249114
138.309600	4900.757464	24.254131
137.892034	4905.522478	24.259149
138.582824	4916.004120	24.264167
138.691667	4924.466992	24.269184
138.735673	4936.392363	24.274202
138.544262	4930.829371	24.279219
138.677445	4941.801175	24.284237
138.715106	4952.261898	24.289255
139.390086	4969.472621	24.294272
139.225715	4969.711358	24.299290
139.173508	4969.862192	24.304307
139.619913	4991.220043	24.309325
139.471099	5001.119701	24.314343
139.940705	5000.865558	24.319360
139.468599	5018.099538	24.324378
139.945687	5023.740750	24.329395
140.077844	5035.039281	24.334413
140.107432	5046.654707	24.339431
140.458573	5058.496586	24.344448
140.258015	5069.249492	24.349466
140.911347	5073.729724	24.354483
141.340324	5094.422567	24.359501
141.532747	5096.881226	24.364519
141.774597	5094.610806	24.369536
141.165678	5097.568580	24.374554
141.672901	5088.331793	24.379571
141.734626	5111.570087	24.384589
141.964280	5120.393801	24.389607
142.192161	5120.827258	24.394624
142.149571	5128.563060	24.399642
142.262777	5121.803575	24.404659
142.281676	5144.693146	24.409677
142.482996	5152.135952	24.414695
142.939421	5154.636705	24.419712
142.672391	5167.626750	24.424730
143.336492	5174.271976	24.429747
143.404022	5176.407544	24.434765
143.449037	5174.497356	24.439783
143.496351	5170.335153	24.444800
143.992375	5178.081081	24.449818
143.935402	5168.218274	24.454835
144.040824	5181.873530	24.459853
144.021546	5187.520785	24.464871
144.255772	5189.423650	24.469888
144.357701	5189.907088	24.474906
144.342531	5196.716494	24.479923
144.700227	5218.338217	24.484941
144.788382	5218.766421	24.489959
145.368511	5227.103181	24.494976
145.075694	5231.152140	24.499994
145.736735	5221.526483	24.505011
145.573236	5226.585451	24.510029
145.470501	5226.973286	24.515047
145.796646	5215.164326	24.520064
145.878715	5223.583647	24.525082
146.182246	5231.267461	24.530099
146.161979	5244.568327	24.535117
146.376788	5246.353136	24.540135
146.592334	5240.869110	24.545152
146.551607	5242.085726	24.550170
146.727257	5237.965981	24.555187
146.960388	5241.534561	24.560205
146.517205	5239.527550	24.565223
147.349557	5249.774442	24.570240
146.805753	5263.586792	24.575258
146.946032	5268.744459	24.580275
147.311518	5268.726417	24.585293
147.439899	5288.220474	24.590311
147.733401	5302.489410	24.595328
147.384245	5302.032236	24.600346
147.527019	5314.490525	24.605363
147.987275	5330.908254	24.610381
147.904870	5332.495000	24.615399
148.255584	5347.477091	24.620416
148.552762	5363.565249	24.625434
148.541417	5365.808618	24.630451
148.813956	5373.683121	24.635469
148.841021	5395.280721	24.640487
149.198763	5400.850635	24.645504
149.088092	5404.641652	24.650522
149.435261	5420.076764	24.655539
149.508433	5421.054156	24.660557
149.414406	5430.400145	24.665575
149.523718	5439.399803	24.670592
149.831747	5462.438879	24.675610
149.625069	5462.747309	24.680627
150.340649	5481.308525	24.685645
150.469163	5490.758324	24.690663
150.845062	5486.056639	24.695680
150.953694	5497.319150	24.700698
151.449926	5502.330453	24.705715
151.860958	5510.874506	24.710733
151.809038	5520.431769	24.715751
151.944140	5519.901307	24.720768
151.873291	5513.824786	24.725786
151.799465	5514.718623	24.730803
152.134909	5509.770046	24.735821
151.991091	5514.540381	24.740839
152.381157	5508.076454	24.745856
152.782405	5533.911862	24.750874
152.808323	5530.166805	24.755891
152.978618	5526.786600	24.760909
152.614954	5537.211810	24.765927
152.914541	5528.737972	24.770944
153.129178	5541.879702	24.775962
153.165307	5549.746363	24.780979
153.376869	5565.086023	24.785997
153.425170	5574.204851	24.791015
153.629272	5565.149852	24.796032
153.822147	5564.488229	24.801050
153.963678	5591.151121	24.806067
154.279572	5593.672000	24.811085
153.932118	5605.382601	24.816103
154.451135	5594.354526	24.821120
154.567789	5603.314562	24.826138
154.591602	5611.375976	24.831155
155.020436	5616.352433	24.836173
155.295873	5617.394359	24.841191
155.546871	5613.612606	24.846208
155.314536	5623.238041	24.851226
155.730666	5619.153016	24.856243
156.218995	5630.010486	24.861261
156.088549	5644.059395	24.866279
156.141355	5640.198302	24.871296
156.256361	5640.578966	24.876314
155.761271	5633.461489	24.881331
156.542022	5649.349334	24.886349
156.570736	5664.758377	24.891367
156.712806	5667.218867	24.896384
156.857100	5678.621383	24.901402
156.764526	5682.065768	24.906419
157.536001	5692.321107	24.911437
157.390266	5698.757392	24.916455
157.630135	5693.377110	24.921472
157.999973	5691.735277	24.926490
158.154136	5693.109679	24.931507
158.079117	5709.348038	24.936525
157.916758	5722.505982	24.941543
158.435010	5722.506857	24.946560
158.311154	5726.568346	24.951578
158.231992	5733.080576	24.956595
158.762299	5744.363374	24.961613
158.793937	5749.188419	24.966631
159.099257	5757.900532	24.971648
159.133393	5783.562028	24.976666
159.107950	5796.085311	24.981683
159.615898	5787.085584	24.986701
159.407472	5810.947904	24.991719
159.614585	5815.809508	24.996736
160.221899	5823.681228	25.001754
160.083062	5825.816750	25.006771
160.571341	5833.082757	25.011789
160.582921	5847.370421	25.016807
161.021606	5849.761619	25.021824
160.970482	5850.721093	25.026842
160.989655	5844.888144	25.031859
161.482864	5852.073910	25.036877
161.451469	5871.154405	25.041895
161.805568	5863.828246	25.046912
162.158595	5870.440783	25.051930
161.653353	5863.898371	25.056947
162.160206	5863.957714	25.061965
161.946927	5873.008285	25.066983
161.946455	5879.704727	25.072000
162.006969	5893.715556	25.077018
162.312762	5899.260113	25.082035
162.496519	5908.739923	25.087053
162.598484	5926.425511	25.092071
162.908818	5920.166881	25.097088
163.258173	5934.809113	25.102106
162.836555	5955.442882	25.107123
163.111516	5958.462877	25.112141
163.061963	5975.507064	25.117159
163.071242	5980.972257	25.122176
163.894817	5989.904000	25.127194
164.435571	6007.552767	25.132211
164.613985	6009.128683	25.137229
164.695863	6021.549285	25.142247
165.010537	6011.185273	25.147264
165.204157	6008.189125	25.152282
164.795050	6017.245044	25.157299
165.142386	6018.949024	25.162317
165.420200	6033.657835	25.167335
165.371786	6036.664890	25.172352
166.043387	6039.506790	25.177370
165.763477	6047.321823	25.182387
166.233751	6058.507432	25.187405
165.979449	6077.997457	25.192423
166.207022	6074.035215	25.197440
166.541965	6071.132180	25.202458
166.524478	6090.066757	25.207475
166.610711	6094.658976	25.212493
166.655041	6101.186295	25.217511
166.868851	6114.385317	25.222528
167.038059	6120.065032	25.227546
167.343293	6122.782041	25.232563
167.551773	6137.902487	25.237581
167.496470	6151.346655	25.242599
168.030103	6150.261671	25.247616
168.169130	6157.350634	25.252634
168.561575	6179.364771	25.257651
168.933269	6176.187560	25.262669
168.806752	6179.340064	25.267687
168.748030	6183.189873	25.272704
168.949622	6177.972878	25.277722
169.086064	6200.060908	25.282739
169.194129	6206.049386	25.287757
169.105152	6216.343938	25.292775
169.609532	6228.812222	25.297792
169.822068	6236.562213	25.302810
169.845470	6248.945122	25.307827
170.231771	6251.959228	25.312845
170.091351	6257.707246	25.317863
170.302126	6269.358474	25.322880
171.009369	6269.945285	25.327898
170.745735	6275.243238	25.332915
171.449122	6274.290114	25.337933
171.172538	6284.434448	25.342951
171.433725	6296.039107	25.347968
171.685431	6298.616766	25.352986
171.361584	6307.732437	25.358003
171.646983	6307.274761	25.363021
171.670586	6316.892095	25.368039
171.457544	6326.791861	25.373056
171.957999	6334.140364	25.378074
172.072844	6363.102425	25.383091
172.573704	6364.917300	25.388109
172.505088	6375.136329	25.393127
172.554524	6393.627881	25.398144
173.064680	6389.979284	25.403162
172.840126	6400.080782	25.408179
173.367886	6416.544824	25.413197
173.721663	6430.686435	25.418215
173.643345	6434.674764	25.423232
174.042765	6430.139773	25.428250
174.364386	6449.912979	25.433267
174.542316	6452.241995	25.438285
174.731041	6460.377502	25.443303
174.719092	6465.994964	25.448320
175.211317	6472.290527	25.453338
174.881644	6486.526210	25.458355
175.174641	6488.113022	25.463373
175.094083	6494.262301	25.468391
175.235491	6512.530833	25.473408
175.583971	6517.469268	25.478426
175.478556	6530.500825	25.483443
175.765872	6546.851494	25.488461
175.745730	6553.802368	25.493479
176.138566	6561.715766	25.498496
176.686138	6569.112739	25.503514
176.524066	6583.033818	25.508531
176.851242	6599.325474	25.513549
177.239473	6608.064213	25.518567
177.086668	6612.867017	25.523584
177.308071	6620.745621	25.528602
177.627037	6637.166878	25.533619
177.683739	6633.571638	25.538637
177.792793	6646.692632	25.543655
178.038849	6667.698530	25.548672
178.289069	6662.697857	25.553690
178.578171	6686.202935	25.558707
178.509322	6691.846078	25.563725
179.085873	6697.213221	25.568743
179.009962	6702.475100	25.573760
179.570907	6715.485552	25.578778
179.589503	6727.765765	25.583795
179.726526	6732.986624	25.588813
179.765533	6726.654469	25.593831
180.098893	6744.670012	25.598848
180.693116	6749.127151	25.603866
180.344845	6768.128706	25.608883
180.702224	6749.753806	25.613901
181.205414	6739.468602	25.618919
181.343949	6737.475636	25.623936
181.389925	6737.822487	25.628954
181.460818	6737.354939	25.633971
181.507260	6738.226526	25.638989
181.792142	6748.435873	25.644007
181.975073	6770.292309	25.649024
182.028546	6770.361790	25.654042
182.067893	6778.289962	25.659059
182.249464	6775.117762	25.664077
182.641098	6777.493801	25.669095
182.415446	6799.086529	25.674112
182.598306	6801.350295	25.679130
182.780079	6813.879952	25.684148
182.692051	6826.416442	25.689165
183.049284	6835.360113	25.694183
183.114873	6857.704334	25.699200
183.786798	6870.044162	25.704218
183.574314	6882.763416	25.709236
183.607289	6899.115683	25.714253
184.027673	6905.957932	25.719271
184.351303	6912.874623	25.724288
184.881276	6921.132227	25.729306
185.037837	6925.077731	25.734324
185.457979	6932.292989	25.739341
185.622913	6921.091428	25.744359
185.688342	6931.367363	25.749376
185.612474	6932.865897	25.754394
185.964890	6944.193718	25.759412
186.183593	6951.260917	25.764429
186.695635	6941.139400	25.769447
186.487411	6946.165952	25.774464
186.819557	6945.113830	25.779482
186.418600	6965.114658	25.784500
186.781200	6969.637121	25.789517
187.088570	6970.417550	25.794535
186.719050	6992.037429	25.799552
187.195780	6997.251430	25.804570
187.579593	7004.112932	25.809588
187.302349	7017.669590	25.814605
187.778664	7032.133728	25.819623
187.924309	7035.386224	25.824640
188.217209	7051.939566	25.829658
188.477229	7065.363399	25.834676
188.634647	7068.017601	25.839693
188.924060	7077.543477	25.844711
189.068121	7096.742350	25.849728
189.391362	7091.953356	25.854746
189.454132	7106.263184	25.859764
189.577410	7126.168451	25.864781
190.083156	7125.605595	25.869799
189.880893	7132.673902	25.874816
189.931509	7143.233249	25.879834
190.059274	7157.572893	25.884852
190.016879	7161.296816	25.889869
190.597271	7179.391530	25.894887
190.442014	7201.431560	25.899904
190.744888	7189.335979	25.904922
191.038145	7209.052560	25.909940
190.903702	7229.108819	25.914957
191.638051	7235.584067	25.919975
191.775896	7259.280980	25.924992
192.148057	7250.569560	25.930010
192.026036	7260.422383	25.935028
192.328152	7280.265116	25.940045
192.784460	7277.049009	25.945063
192.569361	7298.633695	25.950080
192.622769	7301.271474	25.955098
192.995982	7306.976561	25.960116
192.829689	7322.338943	25.965133
193.410472	7328.777340	25.970151
193.770986	7348.802847	25.975168
193.750843	7365.603160	25.980186
194.412397	7376.499614	25.985204
194.384512	7391.485128	25.990221
194.792200	7380.674930	25.995239
194.700427	7398.873142	26.000256
194.844741	7402.923018	26.005274
195.490302	7408.506039	26.010292
195.220081	7415.091954	26.015309
195.514120	7423.788754	26.020327
195.588101	7434.660113	26.025344
195.674809	7439.795606	26.030362
195.944095	7460.137174	26.035380
196.197352	7460.436832	26.040397
196.284330	7472.550959	26.045415
196.487810	7499.014622	26.050432
196.861419	7506.601899	26.055450
196.923277	7507.521433	26.060468
197.054983	7529.445379	26.065485
197.424268	7525.113945	26.070503
197.532365	7544.636235	26.075520
197.765412	7552.164111	26.080538
198.181860	7558.882969	26.085556
198.188108	7576.332410	26.090573
198.879992	7577.020884	26.095591
199.077785	7587.478395	26.100608
199.101265	7592.365929	26.105626
199.267668	7582.657113	26.110644
199.339776	7604.990400	26.115661
199.757594	7615.796844	26.120679
199.619056	7624.805870	26.125696
199.717785	7620.350727	26.130714
200.312660	7637.501024	26.135732
200.075443	7650.711945	26.140749
200.480316	7645.424263	26.145767
200.545254	7663.845678	26.150784
200.422852	7677.958170	26.155802
200.883342	7679.531789	26.160820
200.908440	7700.438246	26.165837
201.215098	7703.580238	26.170855
201.529102	7710.369791	26.175872
201.611742	7722.906578	26.180890
202.099769	7740.640578	26.185908
202.071921	7753.104514	26.190925
202.520872	7746.309199	26.195943
202.306814	7769.989061	26.200960
202.354968	7779.361067	26.205978
202.826237	7773.232601	26.210996
202.872983	7804.441482	26.216013
203.465602	7818.875257	26.221031
203.349048	7826.586483	26.226048
203.535413	7834.668040	26.231066
203.764024	7844.007383	26.236084
203.568949	7857.394324	26.241101
204.306431	7870.315488	26.246119
204.283808	7892.102474	26.251136
204.642798	7900.937921	26.256154
205.103238	7905.071306	26.261172
205.381336	7912.093298	26.266189
205.387902	7930.293790	26.271207
205.875607	7934.992542	26.276224
205.552629	7940.202178	26.281242
206.260558	7954.815998	26.286260
206.172711	7967.055186	26.291277
206.405118	7962.030957	26.296295
206.879105	7977.666885	26.301312
206.759183	7994.171024	26.306330
207.178574	8005.094749	26.311348
207.154155	8003.742157	26.316365
207.256652	8024.373514	26.321383
207.580758	8029.425330	26.326400
207.465497	8035.172379	26.331418
207.759871	8052.024438	26.336436
208.006368	8067.526366	26.341453
208.011626	8075.394171	26.346471
208.558917	8088.345848	26.351488
208.451751	8120.003667	26.356506
209.006086	8124.748907	26.361524
208.970555	8137.769150	26.366541
209.522287	8135.378057	26.371559
209.962300	8154.478389	26.376576
210.180191	8166.530504	26.381594
210.438260	8163.275390	26.386612
210.587194	8183.750840	26.391629
210.949456	8177.802085	26.396647
210.762470	8194.927377	26.401664
210.882920	8209.298708	26.406682
211.007999	8204.340690	26.411700
211.271568	8237.090100	26.416717
211.702142	8242.174984	26.421735
211.876767	8243.430692	26.426752
212.260510	8267.749823	26.431770
212.406492	8274.228054	26.436788
212.408145	8283.864320	26.441805
212.393737	8280.888692	26.446823
212.739459	8303.701907	26.451840
212.635268	8320.995132	26.456858
213.025843	8320.188564	26.461876
213.290731	8348.481762	26.466893
213.256830	8354.105008	26.471911
213.553423	8363.919362	26.476928
213.694312	8376.884539	26.481946
214.104521	8382.048262	26.486964
214.348996	8403.096996	26.491981
214.368158	8414.530218	26.496999
214.746702	8431.959078	26.502016
214.853075	8440.570324	26.507034
215.344393	8449.700160	26.512052
215.406400	8473.806909	26.517069
215.493847	8472.916851	26.522087
215.747619	8493.429522	26.527104
215.989910	8504.243351	26.532122
216.442512	8519.082966	26.537140
216.310869	8534.859311	26.542157
216.460573	8540.631987	26.547175
216.922011	8560.558047	26.552192
217.010246	8576.949772	26.557210
217.193220	8595.124522	26.562228
217.523472	8610.607761	26.567245
217.704919	8628.635641	26.572263
218.055444	8633.110181	26.577280
218.199944	8646.769868	26.582298
218.678543	8659.179002	26.587316
218.423487	8671.042122	26.592333
218.973253	8695.091141	26.597351
219.534644	8691.677390	26.602368
219.475120	8706.561849	26.607386
220.031571	8721.719947	26.612404
220.159909	8727.847464	26.617421
220.222847	8734.537833	26.622439
220.494515	8743.961767	26.627456
220.373513	8763.316391	26.632474
220.795607	8767.748479	26.637492
220.846930	8771.097841	26.642509
220.776949	8794.436070	26.647527
221.455133	8807.441087	26.652544
221.314289	8829.762149	26.657562
221.760708	8831.829188	26.662580
222.027097	8851.718663	26.667597
222.495130	8859.221938	26.672615
222.633714	8875.694099	26.677632
222.958448	8886.011491	26.682650
223.192153	8882.759321	26.687668
223.387990	8903.628436	26.692685
223.356687	8922.555430	26.697703
223.954738	8909.195201	26.702720
223.799305	8932.679079	26.707738
224.008297	8947.166061	26.712756
224.336471	8958.435150	26.717773
224.431480	8964.570045	26.722791
224.482449	8974.618726	26.727808
224.786536	8997.750480	26.732826
225.166347	8996.063436	26.737844
225.027370	9013.087573	26.742861
225.297952	9020.478004	26.747879
225.876198	9022.357617	26.752896
226.039802	9031.718692	26.757914
225.899956	9036.509972	26.762932
226.409334	9058.985442	26.767949
227.314356	9042.422479	26.772967
228.222889	9032.865521	26.777984
228.378550	9021.011101	26.783002
228.806366	9016.811171	26.788020
229.065984	9017.422664	26.793037
229.320603	9015.755181	26.798055
229.177070	8990.406395	26.803072
229.266524	8986.489414	26.808090
229.463199	8979.004666	26.813108
229.452383	8975.511307	26.818125
229.519185	8999.755066	26.823143
229.569662	9001.929712	26.828160
229.646736	9013.075189	26.833178
229.951810	9006.401404	26.838196
230.227760	9013.062662	26.843213
230.388128	9033.493385	26.848231
230.852533	9030.525480	26.853248
230.559031	9048.874322	26.858266
230.702144	9056.034450	26.863284
230.913913	9066.331416	26.868301
231.149434	9078.824901	26.873319
232.117959	9094.193121	26.878336
231.846211	9110.370533	26.883354
231.712701	9111.711245	26.888372
231.865680	9126.096371	26.893389
232.002802	9152.190692	26.898407
232.058846	9163.176734	26.903424
232.462865	9188.892544	26.908442
232.573780	9209.120880	26.913460
232.871441	9229.701932	26.918477
232.631083	9251.281255	26.923495
232.981675	9271.728014	26.928512
233.093223	9300.852120	26.933530
233.609251	9325.612255	26.938548
234.182738	9345.844157	26.943565
234.113737	9368.919884	26.948583
234.991401	9377.874203	26.953600
234.980263	9399.503369	26.958618
235.230408	9412.021164	26.963636
235.497212	9427.631836	26.968653
235.708783	9445.630322	26.973671
236.356957	9456.183791	26.978688
236.562898	9482.717072	26.983706
236.590601	9481.216350	26.988724
236.773649	9485.774116	26.993741
236.873738	9505.166850	26.998759
237.463240	9501.155069	27.003776
237.545494	9515.545154	27.008794
237.514076	9534.642923	27.013812
237.851112	9533.767317	27.018829
238.039469	9557.383484	27.023847
238.481848	9568.119363	27.028864
238.305550	9578.849601	27.033882
238.406679	9599.131962	27.038900
238.912517	9611.032706	27.043917
238.877658	9630.416422	27.048935
239.449188	9645.026111	27.053952
239.795523	9663.328003	27.058970
239.746400	9669.832827	27.063988
240.121832	9687.163309	27.069005
240.260307	9705.063189	27.074023
240.591611	9722.738754	27.079040
241.189795	9738.858433	27.084058
241.415078	9755.806849	27.089076
241.874288	9766.927383	27.094093
241.514511	9777.256531	27.099111
241.964758	9790.870883	27.104128
242.270758	9801.315058	27.109146
242.324121	9822.528860	27.114164
242.588203	9827.503506	27.119181
242.566936	9853.392132	27.124199
242.805127	9869.263989	27.129216
242.994963	9898.041908	27.134234
243.002322	9913.817214	27.139252
243.397288	9932.361158	27.144269
243.495187	9958.776352	27.149287
244.345183	9981.416908	27.154304
244.471589	10005.291556	27.159322
244.591346	10033.081817	27.164340
244.877304	10034.482447	27.169357
244.897044	10043.818295	27.174375
245.465917	10066.190961	27.179392
245.379692	10090.720188	27.184410
245.664873	10113.009866	27.189428
246.277297	10129.763200	27.194445
246.435063	10151.705324	27.199463
246.742076	10168.021805	27.204480
247.233872	10177.842832	27.209498
247.446039	10203.592931	27.214516
247.498031	10208.411451	27.219533
247.734784	10232.634433	27.224551
248.138468	10231.833557	27.229568
248.265865	10249.285682	27.234586
248.528577	10280.992580	27.239604
249.069101	10267.501816	27.244621
248.890802	10293.560252	27.249639
249.480531	10310.230441	27.254656
249.682315	10332.008015	27.259674
249.673142	10338.340699	27.264692
249.953125	10341.419433	27.269709
250.228485	10361.359062	27.274727
250.384197	10371.638708	27.279744
251.041749	10381.646727	27.284762
250.966626	10405.363481	27.289780
251.503552	10407.194777	27.294797
251.472459	10409.781253	27.299815
251.654145	10433.680430	27.304832
252.056242	10438.998061	27.309850
252.042576	10463.224737	27.314868
252.704525	10472.741410	27.319885
252.857083	10484.108509	27.324903
252.857852	10502.480676	27.329920
252.974879	10519.637274	27.334938
253.005488	10542.072842	27.339956
253.565053	10560.124225	27.344973
253.545449	10573.636713	27.349991
253.965524	10596.073634	27.355008
254.447793	10603.123378	27.360026
254.677414	10622.159269	27.365044
254.752570	10635.001507	27.370061
254.791419	10653.577530	27.375079
255.444487	10670.412350	27.380096
255.985999	10688.729633	27.385114
256.253406	10692.405833	27.390132
256.915583	10704.073965	27.395149
256.821600	10715.707989	27.400167
256.852362	10730.522602	27.405184
257.288676	10741.922972	27.410202
257.590460	10751.417747	27.415220
257.814417	10759.331978	27.420237
257.993958	10788.960087	27.425255
258.107001	10786.289479	27.430272
258.577105	10813.027370	27.435290
258.594944	10827.711522	27.440308
258.799589	10840.249174	27.445325
258.940127	10862.447717	27.450343
258.881774	10886.622379	27.455360
259.282004	10902.193245	27.460378
259.332981	10927.036843	27.465396
259.758522	10941.220095	27.470413
260.193455	10965.817205	27.475431
260.744124	10988.769871	27.480448
261.568219	10981.833829	27.485466
261.379451	10995.395302	27.490484
262.089007	11019.095173	27.495501
262.288250	11026.274054	27.500519
262.493339	11024.595758	27.505536
263.094860	11034.581273	27.510554
263.122163	11055.871403	27.515572
263.274062	11052.240258	27.520589
263.509349	11062.715473	27.525607
263.119585	11070.340468	27.530624
263.451215	11071.595399	27.535642
263.693658	11093.405371	27.540660
263.955149	11112.228626	27.545677
264.282637	11120.995056	27.550695
264.662742	11141.212985	27.555712
264.950885	11145.529801	27.560730
264.965713	11154.920244	27.565748
265.137672	11175.108826	27.570765
265.183920	11188.640094	27.575783
265.732779	11210.672926	27.580800
265.713066	11219.420775	27.585818
266.055536	11251.080596	27.590836
266.243170	11261.073797	27.595853
266.346809	11286.213789	27.600871
266.553280	11319.413082	27.605888
267.288168	11320.791470	27.610906
267.609594	11352.308858	27.615924
268.001149	11362.584643	27.620941
268.021801	11384.097460	27.625959
268.246891	11405.107644	27.630976
268.802443	11414.555893	27.635994
268.689605	11439.961848	27.641012
269.154677	11449.739960	27.646029
269.527389	11465.164678	27.651047
269.666577	11485.730788	27.656064
270.010294	11499.501411	27.661082
270.172141	11523.932813	27.666100
270.620955	11539.871241	27.671117
271.068152	11548.406329	27.676135
271.544643	11556.915502	27.681152
272.110439	11563.183023	27.686170
272.042283	11593.579842	27.691188
272.298373	11604.595200	27.696205
272.538812	11612.218396	27.701223
272.363671	11632.216756	27.706240
272.687284	11649.350955	27.711258
273.110964	11665.190612	27.716276
273.329465	11675.251776	27.721293
273.671305	11699.272839	27.726311
273.897396	11723.710064	27.731328
274.315123	11721.467699	27.736346
274.162199	11750.924794	27.741364
274.593800	11770.788647	27.746381
275.059226	11783.759537	27.751399
275.017331	11806.401175	27.756416
275.225788	11835.381706	27.761434
275.935014	11859.696883	27.766452
275.953421	11875.990773	27.771469
276.176872	11894.577854	27.776487
276.255025	11922.614150	27.781504
276.870395	11933.893418	27.786522
276.834335	11958.782490	27.791540
276.778982	11995.653114	27.796557
277.166066	12004.120120	27.801575
277.518118	12031.168638	27.806592
277.859414	12054.800147	27.811610
278.884858	12057.156709	27.816628
280.275434	12052.156289	27.821645
280.534741	12062.019548	27.826663
280.639211	12066.205732	27.831680
281.072618	12056.256876	27.836698
281.009650	12062.769459	27.841716
281.205987	12069.467201	27.846733
281.500250	12060.869344	27.851751
281.247171	12064.629830	27.856768
281.379181	12066.519783	27.861786
281.367751	12073.805551	27.866804
281.565589	12093.015620	27.871821
281.814608	12102.451377	27.876839
281.830059	12123.225210	27.881856
282.329713	12134.895964	27.886874
282.252928	12157.412830	27.891892
282.534233	12184.472506	27.896909
283.152497	12208.661656	27.901927
282.797432	12236.326015	27.906944
283.337805	12259.007949	27.911962
283.665919	12287.849450	27.916980
283.978543	12300.729436	27.921997
284.055647	12329.132657	27.927015
283.901997	12360.908313	27.932032
284.557872	12387.267933	27.937050
285.169819	12409.954820	27.942068
285.436838	12435.256631	27.947085
285.852198	12461.299922	27.952103
286.468867	12473.144739	27.957120
287.021588	12483.303115	27.962138
287.352173	12503.485499	27.967156
287.981130	12504.115024	27.972173
288.417527	12522.944034	27.977191
288.065835	12543.011283	27.982208
288.458268	12547.122972	27.987226
288.634632	12569.311812	27.992244
288.889299	12577.605434	27.997261
289.146598	12586.839653	28.002279
289.307018	12612.239037	28.007296
289.385099	12636.703292	28.012314
289.670919	12648.319976	28.017332
289.910812	12667.910944	28.022349
289.975189	12692.190135	28.027367
290.080241	12721.383851	28.032384
290.493477	12734.650002	28.037402
290.881233	12766.807374	28.042420
291.059015	12794.247899	28.047437
291.956438	12813.282827	28.052455
291.713103	12849.076006	28.057472
292.056640	12860.743476	28.062490
292.447814	12898.821170	28.067508
292.911148	12921.221982	28.072525
293.746002	12931.562292	28.077543
293.636972	12958.563552	28.082560
294.100667	12963.172987	28.087578
294.003250	12988.598352	28.092596
294.094153	13008.429184	28.097613
294.639739	13017.123582	28.102631
294.807896	13041.904242	28.107648
294.981297	13057.506892	28.112666
295.247451	13079.222467	28.117684
295.627531	13104.546729	28.122701
296.307421	13120.492599	28.127719
296.217749	13148.969979	28.132736
296.425093	13169.833513	28.137754
296.615158	13189.767834	28.142772
296.959587	13212.428899	28.147789
297.367751	13227.250635	28.152807
297.714314	13261.469419	28.157824
297.917489	13277.563265	28.162842
297.618396	13306.628112	28.167860
298.142440	13344.289109	28.172877
298.694748	13367.472420	28.177895
298.972662	13392.332583	28.182912
299.218355	13420.416073	28.187930
299.605526	13444.875456	28.192948
300.053684	13474.288583	28.197965
300.444376	13488.488245	28.202983
301.202365	13515.540138	28.208000
301.347399	13529.771613	28.213018
301.653328	13554.093967	28.218036
301.774838	13576.854865	28.223053
302.557150	13580.624364	28.228071
302.484078	13606.127757	28.233088
303.086561	13618.635590	28.238106
303.353262	13639.548459	28.243124
303.271089	13656.657600	28.248141
303.779349	13668.972380	28.253159
303.970985	13691.473914	28.258176
304.006867	13709.643922	28.263194
304.410206	13733.044692	28.268212
304.494163	13763.410669	28.273229
304.836741	13777.816543	28.278247
304.993927	13809.382522	28.283264
305.756592	13828.159180	28.288282
306.122871	13847.330348	28.293300
306.265270	13864.328456	28.298317
306.920703	13880.442072	28.303335
307.354774	13904.126219	28.308352
307.647525	13923.789491	28.313370
307.943408	13933.778910	28.318388
308.071881	13959.557284	28.323405
308.538040	13969.136615	28.328423
308.472308	13992.143766	28.333440
308.906372	14013.381170	28.338458
309.184533	14028.041187	28.343476
309.147241	14048.627573	28.348493
310.216280	14064.183658	28.353511
310.482924	14091.368515	28.358528
310.849545	14100.182296	28.363546
311.204526	14108.147238	28.368564
311.117661	14133.591617	28.373581
311.525772	14133.773079	28.378599
311.962300	14158.688324	28.383616
311.852309	14171.104313	28.388634
312.441576	14180.285214	28.393652
312.853137	14207.291117	28.398669
312.769523	14222.878358	28.403687
313.062611	14242.051159	28.408704
313.085866	14258.404581	28.413722
313.415581	14283.707537	28.418740
313.265499	14314.961118	28.423757
314.160660	14333.960042	28.428775
313.884926	14360.857403	28.433792
314.531326	14390.715787	28.438810
314.856717	14411.483580	28.443828
315.067038	14446.373730	28.448845
315.557180	14468.954887	28.453863
315.785360	14491.577534	28.458880
316.175887	14514.728056	28.463898
316.907927	14540.564820	28.468916
317.675037	14557.645096	28.473933
318.189818	14573.723217	28.478951
318.588311	14586.047773	28.483968
318.624923	14598.188729	28.488986
319.496325	14606.405437	28.494004
319.497330	14609.636877	28.499021
319.739747	14624.257897	28.504039
319.856687	14636.715735	28.509056
319.918396	14655.205022	28.514074
320.248236	14675.415299	28.519092
320.569352	14694.054883	28.524109
320.802858	14716.017604	28.529127
320.970912	14737.311402	28.534144
321.065840	14757.238329	28.539162
321.491392	14780.344309	28.544180
321.829850	14802.294363	28.549197
322.084332	14823.293165	28.554215
322.194626	14850.755321	28.559232
322.454383	14883.484096	28.564250
322.852345	14908.957390	28.569268
322.850485	14949.810081	28.574285
323.509510	14981.564387	28.579303
323.915328	15012.396402	28.584320
324.039552	15040.941020	28.589338
324.950429	15058.429673	28.594356
324.958540	15085.408135	28.599373
325.389258	15113.034220	28.604391
325.978369	15149.662121	28.609408
326.065916	15169.684738	28.614426
326.416882	15183.179840	28.619444
326.421808	15209.438684	28.624461
327.002735	15236.287542	28.629479
327.458818	15258.156029	28.634496
327.779419	15286.848712	28.639514
327.991125	15299.952304	28.644532
328.196582	15321.909439	28.649549
329.300933	15333.507641	28.654567
329.599471	15345.096997	28.659584
329.704496	15350.351731	28.664602
330.276938	15367.274899	28.669620
330.266650	15389.466875	28.674637
330.317188	15408.250532	28.679655
331.037075	15421.190673	28.684672
330.880422	15443.882945	28.689690
331.114967	15460.602629	28.694708
331.435303	15489.712202	28.699725
331.673917	15519.990383	28.704743
332.148910	15537.272326	28.709760
332.151197	15569.378738	28.714778
332.523616	15589.840580	28.719796
332.453981	15632.304656	28.724813
333.079117	15655.696340	28.729831
333.549761	15685.121451	28.734848
333.923828	15709.256867	28.739866
334.514084	15731.884652	28.744884
334.852032	15760.207003	28.749901
335.456606	15790.733451	28.754919
335.763394	15814.498313	28.759936
335.946104	15838.272947	28.764954
336.344541	15861.859715	28.769972
336.408236	15890.913520	28.774989
336.707495	15923.008373	28.780007
337.008815	15939.655542	28.785024
337.208784	15982.276013	28.790042
337.461835	15998.711282	28.795060
338.075008	16030.404603	28.800077
338.345344	16061.948911	28.805095
338.366997	16091.219020	28.810112
338.817876	16126.584032	28.815130
339.693186	16145.728227	28.820148
339.746420	16178.923723	28.825165
340.011428	16199.439711	28.830183
340.714520	16227.432514	28.835200
340.941859	16262.495311	28.840218
341.287284	16291.845486	28.845236
341.486563	16317.648317	28.850253
341.936337	16339.294963	28.855271
342.271586	16363.109475	28.860288
342.907657	16392.195433	28.865306
343.341629	16401.423489	28.870324
343.700016	16431.485178	28.875341
343.746158	16453.857270	28.880359
344.540359	16473.280721	28.885376
344.640874	16513.126645	28.890394
345.293000	16515.439339	28.895412
345.559716	16549.412557	28.900429
345.810549	16562.452826	28.905447
346.078448	16573.676765	28.910464
346.436152	16603.551908	28.915482
346.750865	16616.583813	28.920500
347.373302	16639.240284	28.925517
347.474183	16656.959848	28.930535
347.651548	16665.436307	28.935552
347.823224	16694.244117	28.940570
348.054208	16708.393883	28.945588
348.351805	16734.421684	28.950605
348.618431	16764.225831	28.955623
349.169027	16789.720136	28.960640
349.195981	16821.443159	28.965658
349.784293	16843.425102	28.970676
349.904697	16872.868734	28.975693
350.547646	16910.085512	28.980711
351.262972	16928.258807	28.985728
351.441581	16954.584270	28.990746
351.470365	16977.371669	28.995764
351.838162	17002.457493	29.000781
352.071805	17032.315835	29.005799
352.564659	17057.787110	29.010816
352.972969	17092.385179	29.015834
353.069314	17122.534458	29.020852
353.579632	17147.441710	29.025869
353.887253	17175.561462	29.030887
354.178323	17193.621785	29.035904
354.523082	17231.434076	29.040922
354.911023	17269.163595	29.045940
355.396784	17289.371650	29.050957
355.633985	17316.315922	29.055975
356.285136	17345.464264	29.060992
356.537437	17379.739425	29.066010
356.855029	17405.707296	29.071028
357.261320	17431.674068	29.076045
357.200845	17468.262187	29.081063
357.973470	17487.830710	29.086080
358.197081	17522.427678	29.091098
358.595072	17554.811554	29.096116
359.273302	17577.477441	29.101133
359.661924	17600.635173	29.106151
360.487489	17618.306884	29.111168
360.610125	17643.770801	29.116186
360.829527	17658.860075	29.121204
361.142538	17680.690237	29.126221
361.238568	17709.477344	29.131239
361.819492	17719.927638	29.136256
361.978409	17755.768883	29.141274
362.321998	17779.976567	29.146292
362.773645	17808.143411	29.151309
363.105787	17841.066722	29.156327
363.463776	17858.871096	29.161344
363.968293	17892.015075	29.166362
364.204671	17915.299506	29.171380
364.719568	17927.789595	29.176397
364.810682	17970.811427	29.181415
365.386699	17980.091025	29.186432
365.743711	18011.100098	29.191450
365.869676	18048.789403	29.196468
366.313964	18072.713384	29.201485
366.636648	18095.320548	29.206503
366.874089	18112.687332	29.211520
366.884683	18150.096052	29.216538
367.211132	18166.385313	29.221556
367.902695	18198.510361	29.226573
367.977207	18239.565470	29.231591
368.683863	18260.543151	29.236608
369.118512	18283.058727	29.241626
369.581282	18315.988212	29.246644
369.588301	18334.153793	29.251661
370.014537	18368.803428	29.256679
370.224554	18393.821958	29.261696
370.471037	18426.475898	29.266714
370.905593	18465.787561	29.271732
371.576557	18494.628993	29.276749
371.964839	18530.074433	29.281767
372.647282	18555.713242	29.286784
373.174346	18586.194769	29.291802
373.525980	18600.107932	29.296820
374.345856	18622.835066	29.301837
374.372102	18655.644273	29.306855
375.048849	18667.119753	29.311872
374.997454	18697.341299	29.316890
375.485931	18722.797110	29.321908
375.704729	18739.458475	29.326925
375.782968	18775.492885	29.331943
376.168752	18799.945447	29.336960
376.711672	18834.786986	29.341978
377.308856	18854.617889	29.346996
378.074548	18861.445999	29.352013
378.262551	18887.162966	29.357031
378.664519	18913.001400	29.362048
378.548503	18933.850836	29.367066
378.763935	18956.235775	29.372084
379.396903	18984.753049	29.377101
379.886648	19026.811061	29.382119
380.116750	19053.486227	29.387136
381.029567	19064.321192	29.392154
381.137478	19086.232471	29.397172
381.749542	19113.760720	29.402189
381.437861	19145.593626	29.407207
381.919204	19172.648677	29.412224
382.361229	19213.652902	29.417242
382.473169	19235.627139	29.422260
383.000833	19269.577125	29.427277
383.190377	19305.303657	29.432295
383.461132	19343.149015	29.437312
384.121646	19375.592496	29.442330
384.078133	19411.132370	29.447348
384.631865	19451.841047	29.452365
385.019790	19484.190776	29.457383
385.714425	19513.659522	29.462400
386.185176	19553.705635	29.467418
386.316873	19579.046452	29.472436
386.840990	19601.748126	29.477453
387.118925	19631.811900	29.482471
387.468908	19659.383662	29.487488
387.646485	19686.738431	29.492506
388.329782	19713.059403	29.497524
388.613083	19739.930042	29.502541
388.612208	19780.542102	29.507559
389.303335	19811.040831	29.512576
389.258625	19853.325619	29.517594
389.409029	19884.858802	29.522612
390.219186	19915.682905	29.527629
390.980662	19950.597633	29.532647
391.632749	19971.821392	29.537664
392.194715	20001.954411	29.542682
392.375097	20040.486023	29.547700
392.701507	20061.249920	29.552717
393.108480	20096.841234	29.557735
393.582172	20120.759345	29.562752
393.941255	20151.220297	29.567770
394.193785	20188.351209	29.572788
394.462539	20209.533997	29.577805
394.625531	20250.987037	29.582823
395.129102	20282.056021	29.587840
395.471038	20329.254452	29.592858
395.845227	20360.268999	29.597876
396.604900	20388.099647	29.602893
396.843290	20426.930886	29.607911
397.453881	20458.041049	29.612928
397.941610	20484.763836	29.617946
398.074806	20520.186314	29.622964
398.569437	20558.039097	29.627981
398.827118	20592.314155	29.632999
399.250977	20619.001671	29.638016
399.657781	20656.117375	29.643034
399.987294	20688.858099	29.648052
400.556201	20730.115808	29.653069
400.647848	20765.596650	29.658087
401.225579	20799.656565	29.663104
401.790143	20832.086067	29.668122
402.281908	20871.836476	29.673140
402.425776	20900.965597	29.678157
402.695759	20941.897408	29.683175
403.006736	20987.936384	29.688192
403.301301	21014.441197	29.693210
403.856778	21058.804093	29.698228
404.645880	21093.919371	29.703245
404.680467	21142.474990	29.708263
405.191288	21169.404755	29.713280
405.785611	21201.790113	29.718298
405.883870	21239.594286	29.723316
406.313693	21271.467303	29.728333
406.678383	21315.691208	29.733351
406.994937	21353.912149	29.738368
407.349653	21388.583016	29.743386
407.697987	21424.290640	29.748404
408.947250	21440.607178	29.753421
409.417307	21468.270884	29.758439
410.064386	21495.993854	29.763456
410.373985	21510.229765	29.768474
410.604303	21545.915515	29.773492
410.996186	21566.226380	29.778509
411.252529	21591.467883	29.783527
411.117325	21618.530495	29.788544
411.547008	21659.893948	29.793562
411.774684	21694.652676	29.798580
412.298339	21718.215965	29.803597
412.503965	21770.966964	29.808615
413.089213	21812.839231	29.813632
413.400444	21843.116155	29.818650
413.369945	21892.850094	29.823668
413.949009	21929.297095	29.828685
414.480627	21974.111363	29.833703
415.382404	22008.828744	29.838720
415.797721	22047.928774	29.843738
416.492494	22084.846014	29.848756
417.101359	22110.081796	29.853773
417.793936	22152.188323	29.858791
417.736292	22181.994608	29.863808
418.566962	22205.449848	29.868826
418.708350	22242.067336	29.873844
418.859483	22269.470580	29.878861
419.957702	22276.735551	29.883879
420.354617	22321.536827	29.888896
420.697421	22337.309570	29.893914
421.278083	22363.367016	29.898932
421.696744	22396.813819	29.903949
422.266408	22419.806100	29.908967
422.341598	22445.711871	29.913984
422.535453	22464.517998	29.919002
422.976432	22497.460527	29.924020
423.042970	22531.541840	29.929037
423.809925	22555.988357	29.934055
423.788356	22600.209666	29.939072
424.546208	22633.520224	29.944090
425.059157	22672.151776	29.949108
425.413605	22705.457449	29.954125
425.823856	22741.798536	29.959143
425.707574	22780.263598	29.964160
426.321187	22810.708434	29.969178
426.510673	22859.580964	29.974196
427.180721	22897.661098	29.979213
427.508962	22938.610065	29.984231
427.875490	22978.911886	29.989248
428.719965	23016.710103	29.994266
428.603651	23057.070938	29.999284
429.106715	23099.600862	30.004301
429.458868	23138.252868	30.009319
429.730946	23178.571032	30.014336
430.529519	23211.302900	30.019354
430.974113	23254.231660	30.024372
431.372097	23294.384339	30.029389
432.047317	23320.348741	30.034407
432.501734	23349.637685	30.039424
432.968538	23386.683294	30.044442
433.006293	23415.039975	30.049460
433.929456	23441.610178	30.054477
434.381980	23481.794813	30.059495
434.718983	23508.265539	30.064512
435.623230	23532.056035	30.069530
435.778643	23559.792439	30.074548
435.955820	23603.901378	30.079565
436.721338	23623.856825	30.084583
436.970664	23655.494805	30.089600
437.549131	23673.272231	30.094618
437.924269	23712.294548	30.099636
438.243795	23741.202409	30.104653
438.588063	23772.718370	30.109671
438.623176	23811.250810	30.114688
439.143646	23852.762275	30.119706
439.775126	23889.544935	30.124724
440.023366	23937.642622	30.129741
440.580066	23977.317235	30.134759
440.691705	24017.722166	30.139776
441.172732	24053.620952	30.144794
441.650617	24102.302472	30.149812
441.832365	24149.370040	30.154829
442.642472	24193.116670	30.159847
443.070153	24240.764467	30.164864
443.272179	24270.065385	30.169882
443.763217	24317.953812	30.174900
444.429234	24359.196851	30.179917
445.024577	24397.721794	30.184935
445.397111	24435.790789	30.189952
445.907940	24468.510440	30.194970
446.599569	24512.296518	30.199988
447.015455	24553.778421	30.205005
447.367435	24598.940664	30.210023
447.527709	24643.393893	30.215040
448.129204	24677.556840	30.220058
448.625768	24714.634670	30.225076
448.832770	24759.234386	30.230093
449.618724	24802.015252	30.235111
449.993552	24836.012201	30.240128
450.662849	24869.251759	30.245146
451.077491	24916.958005	30.250164
451.285539	24951.960157	30.255181
451.917075	24993.070109	30.260199
452.209960	25035.254264	30.265216
452.996338	25070.637976	30.270234
453.279588	25113.235869	30.275252
453.338114	25153.936513	30.280269
454.016870	25187.060212	30.285287
454.244425	25236.932055	30.290304
454.970110	25273.606792	30.295322
455.446554	25312.215119	30.300340
455.810185	25350.249108	30.305357
456.318092	25380.058706	30.310375
456.272403	25432.450657	30.315392
456.587855	25469.455106	30.320410
456.974318	25509.916915	30.325428
457.180800	25558.412926	30.330445
457.753758	25601.334641	30.335463
457.952524	25652.887189	30.340480
458.289759	25709.950476	30.345498
458.905213	25764.376234	30.350516
459.361613	25819.189113	30.355533
460.188717	25859.565845	30.360551
461.071911	25907.509993	30.365568
461.849712	25951.654972	30.370586
462.431998	25982.945146	30.375604
462.891999	26022.450382	30.380621
463.184501	26065.255732	30.385639
463.650461	26094.502182	30.390656
464.598802	26119.046611	30.395674
465.130251	26155.811037	30.400692
465.627623	26190.535029	30.405709
466.221766	26208.203284	30.410727
466.545885	26255.560812	30.415744
466.799946	26276.417251	30.420762
467.571488	26314.056867	30.425780
467.658174	26341.719229	30.430797
468.052020	26384.622730	30.435815
468.351818	26420.094036	30.440832
469.064666	26462.152008	30.445850
469.454313	26500.316932	30.450868
469.551176	26547.113562	30.455885
470.356127	26584.754005	30.460903
470.202151	26630.924336	30.465920
471.064070	26677.273297	30.470938
471.377951	26720.418904	30.475956
471.750936	26764.713334	30.480973
472.296444	26806.137868	30.485991
472.470497	26853.833835	30.491008
473.186096	26902.248058	30.496026
473.896501	26956.687148	30.501044
473.872267	27008.036903	30.506061
474.718886	27046.755873	30.511079
475.172390	27096.792871	30.516096
475.441796	27143.786704	30.521114
476.295197	27190.756969	30.526132
476.349427	27242.925374	30.531149
477.014626	27282.587735	30.536167
477.542752	27336.809757	30.541184
477.936146	27376.126442	30.546202
478.356939	27425.763129	30.551220
478.439290	27479.752528	30.556237
479.404513	27517.757254	30.561255
480.003636	27573.640634	30.566272
480.287942	27623.376883	30.571290
480.609309	27661.386823	30.576308
480.948445	27706.414080	30.581325
481.682188	27758.882443	30.586343
482.118508	27805.375723	30.591360
482.745408	27835.236310	30.596378
483.310848	27874.919169	30.601396
483.971870	27914.796480	30.606413
485.458583	27924.810272	30.611431
485.940461	27956.599321	30.616448
486.102750	27987.596293	30.621466
486.726717	28009.588135	30.626484
487.297171	28031.828054	30.631501
487.677064	28056.474676	30.636519
488.520577	28082.761957	30.641536
489.046124	28112.580900	30.646554
489.372334	28133.414851	30.651572
489.778929	28166.981218	30.656589
490.383933	28196.133693	30.661607
490.492166	28222.032498	30.666624
490.231317	28259.165886	30.671642
491.131112	28300.789945	30.676660
491.538262	28340.927791	30.681677
491.896426	28381.239003	30.686695
491.952188	28415.673329	30.691712
492.611853	28461.994240	30.696730
492.923660	28510.836903	30.701748
493.143062	28570.711232	30.706765
493.540031	28609.007612	30.711783
493.623658	28665.403937	30.716800
493.992530	28729.612304	30.721818
495.105972	28776.493748	30.726836
495.307575	28843.595728	30.731853
495.724686	28900.136725	30.736871
496.506380	28960.310580	30.741888
496.780864	29017.582282	30.746906
497.462826	29070.890488	30.751924
497.496768	29140.860178	30.756941
498.165364	29190.357202	30.761959
498.943150	29253.389897	30.766976
499.545378	29316.439771	30.771994
500.264005	29370.994405	30.777012
500.148341	29432.510664	30.782029
501.347494	29481.679785	30.787047
501.894222	29539.352790	30.792064
502.288057	29595.400332	30.797082
503.231143	29636.366899	30.802100
503.338009	29697.063878	30.807117
504.040770	29744.834616	30.812135
504.468414	29792.869956	30.817152
504.494651	29849.216475	30.822170
504.924848	29900.791373	30.827188
505.626953	29950.803867	30.832205
506.047107	30006.492453	30.837223
506.815674	30061.968127	30.842240
507.731683	30104.513032	30.847258
508.579241	30138.452925	30.852276
509.244419	30179.641643	30.857293
509.527970	30217.668308	30.862311
510.132346	30242.980659	30.867328
510.445406	30285.057870	30.872346
511.310363	30320.435853	30.877364
511.815315	30353.214080	30.882381
512.107576	30386.692913	30.887399
512.375809	30425.720129	30.892416
512.646004	30469.180520	30.897434
513.508667	30496.948566	30.902452
513.632040	30556.724118	30.907469
513.913515	30602.849737	30.912487
514.631813	30658.647503	30.917504
514.730519	30698.398990	30.922522
515.513988	30744.339445	30.927540
515.912346	30804.095736	30.932557
516.573461	30853.351551	30.937575
516.990929	30911.934166	30.942592
517.257048	30970.845283	30.947610
517.961620	31015.992113	30.952628
518.166039	31079.510905	30.957645
518.562895	31127.977461	30.962663
519.340362	31175.642761	30.967680
519.729853	31241.446421	30.972698
520.374783	31293.653466	30.977716
521.235804	31338.185218	30.982733
521.763828	31395.323980	30.987751
522.481500	31447.817816	30.992768
523.053655	31493.652181	30.997786
524.788862	31516.716906	31.002804
524.997757	31563.597570	31.007821
525.398039	31595.179748	31.012839
526.357662	31627.399494	31.017856
526.557925	31679.339725	31.022874
526.883119	31711.121649	31.027892
527.295445	31745.451016	31.032909
527.575465	31777.782463	31.037927
528.137183	31828.352644	31.042944
528.422878	31884.185658	31.047962
529.392570	31919.085444	31.052980
530.647724	31950.492729	31.057997
530.903624	31984.194973	31.063015
531.797926	31999.396782	31.068032
532.193578	32040.497558	31.073050
532.624543	32076.243216	31.078068
533.159910	32108.747426	31.083085
533.460502	32143.880367	31.088103
533.783155	32177.689012	31.093120
533.874760	32225.758208	31.098138
534.383657	32260.104789	31.103156
535.091557	32310.847041	31.108173
535.279522	32358.603370	31.113191
535.906640	32410.758479	31.118208
536.164347	32457.172074	31.123226
536.411067	32504.184942	31.128244
537.135329	32551.760253	31.133261
537.549100	32593.212597	31.138279
537.701001	32637.589710	31.143296
538.410759	32712.709555	31.148314
539.185666	32742.215080	31.153332
539.541607	32801.540870	31.158349
539.722130	32866.756950	31.163367
540.242468	32902.942551	31.168384
540.921600	32974.484023	31.173402
541.906833	33015.614689	31.178420
542.306432	33072.390377	31.183437
542.975084	33118.466096	31.188455
543.759135	33160.087868	31.193472
543.804379	33233.348705	31.198490
544.790102	33277.474920	31.203508
545.175993	33330.959198	31.208525
545.437930	33388.281230	31.213543
545.964544	33441.541681	31.218560
546.665958	33507.151784	31.223578
546.922898	33565.876581	31.228596
547.785594	33617.406846	31.233613
548.140144	33672.090503	31.238631
548.518709	33732.986060	31.243648
549.066211	33801.538088	31.248666
549.714581	33858.026199	31.253684
550.231993	33917.230948	31.258701
550.244578	33991.827630	31.263719
551.127208	34052.086031	31.268736
552.043905	34121.241075	31.273754
552.799150	34176.961311	31.278772
553.796915	34228.878671	31.283789
554.339321	34277.406945	31.288807
554.960649	34319.342876	31.293824
555.111074	34378.957684	31.298842
556.138824	34418.812902	31.303860
557.324195	34457.564841	31.308877
557.998816	34510.772041	31.313895
559.065025	34538.695787	31.318912
559.302173	34579.293700	31.323930
559.773745	34609.844024	31.328948
560.381401	34656.482328	31.333965
560.525396	34704.241371	31.338983
561.110264	34740.341881	31.344000
561.284210	34787.795290	31.349018
561.393112	34833.775752	31.354036
562.351572	34880.519608	31.359053
562.224294	34936.732926	31.364071
562.932978	34984.678710	31.369088
563.654080	35043.451446	31.374106
564.228159	35107.033995	31.379124
564.690320	35161.134715	31.384141
565.238374	35222.787504	31.389159
565.918061	35280.115722	31.394176
566.174556	35329.085144	31.399194
566.589107	35384.942510	31.404212
567.096746	35433.747694	31.409229
567.262802	35506.136921	31.414247
567.952003	35560.182276	31.419264
568.481274	35623.766043	31.424282
568.985273	35687.361961	31.429300
569.615617	35744.152570	31.434317
570.020869	35812.265708	31.439335
570.602785	35876.988201	31.444352
571.364452	35941.056420	31.449370
572.013260	36010.027055	31.454388
572.594662	36061.340093	31.459405
573.006027	36140.584170	31.464423
573.717090	36191.810739	31.469440
574.180300	36254.256515	31.474458
574.739715	36317.287883	31.479476
575.386313	36379.753791	31.484493
575.852003	36455.124880	31.489511
576.444132	36519.854531	31.494528
577.145305	36586.714418	31.499546
577.808745	36649.000487	31.504564
578.590188	36716.519748	31.509581
579.162134	36786.530622	31.514599
579.569475	36845.971388	31.519616
580.389257	36901.731421	31.524634
581.019561	36958.672774	31.529652
581.869754	37025.802353	31.534669
582.473362	37080.593078	31.539687
583.168163	37121.961465	31.544704
583.879540	37188.240327	31.549722
584.723384	37248.344570	31.554740
585.355751	37289.843141	31.559757
585.693191	37345.301485	31.564775
586.368351	37399.164217	31.569792
587.014618	37454.814969	31.574810
587.506948	37505.947937	31.579828
588.164906	37553.158635	31.584845
588.307692	37624.422295	31.589863
588.953903	37672.144475	31.594880
589.633357	37726.321335	31.599898
590.879902	37770.438394	31.604916
591.593225	37814.072868	31.609933
592.055262	37859.256413	31.614951
592.771007	37907.261458	31.619968
593.543711	37955.432587	31.624986
593.953025	38010.105907	31.630004
594.324802	38064.835838	31.635021
594.756598	38117.564939	31.640039
595.154362	38154.541433	31.645056
595.622476	38225.121950	31.650074
595.787445	38286.260419	31.655092
596.977374	38334.727263	31.660109
597.328354	38399.983453	31.665127
597.754955	38455.041769	31.670144
598.468640	38510.540196	31.675162
599.012650	38564.966797	31.680180
599.705614	38604.316075	31.685197
600.207353	38672.770719	31.690215
600.848071	38709.763345	31.695232
601.350874	38766.731099	31.700250
601.789946	38825.766952	31.705268
602.520233	38866.028608	31.710285
602.593633	38938.691721	31.715303
603.135417	39000.841847	31.720320
603.718842	39059.196402	31.725338
603.774659	39135.032618	31.730356
604.687241	39198.663426	31.735373
605.121845	39283.636236	31.740391
605.843507	39356.760835	31.745408
606.527057	39425.872344	31.750426
606.805106	39504.705581	31.755444
607.623071	39571.522400	31.760461
608.269017	39648.213055	31.765479
608.956763	39723.340988	31.770496
609.734762	39796.379657	31.775514
609.974608	39875.665382	31.780532
610.583167	39939.225953	31.785549
611.362854	40031.958069	31.790567
612.227048	40101.046701	31.795584
612.809577	40182.444421	31.800602
613.094446	40246.644311	31.805620
613.838654	40317.183227	31.810637
614.285454	40400.407647	31.815655
614.851330	40490.993775	31.820672
615.623125	40562.371416	31.825690
616.245149	40642.017731	31.830708
617.302562	40727.871548	31.835725
617.863904	40790.140199	31.840743
618.448245	40865.746954	31.845760
618.988152	40928.997272	31.850778
619.487006	41015.537596	31.855796
620.341284	41083.677675	31.860813
621.662184	41132.346121	31.865831
623.025659	41181.389571	31.870848
624.163410	41228.999300	31.875866
624.728664	41279.829204	31.880884
625.358709	41322.684803	31.885901
625.667353	41388.591560	31.890919
626.342373	41420.142165	31.895936
626.958989	41469.765883	31.900954
627.301078	41517.127778	31.905972
628.094881	41567.016897	31.910989
628.528239	41630.535949	31.916007
628.718810	41685.085558	31.921024
629.330347	41733.774056	31.926042
629.658133	41811.466594	31.931060
630.479297	41863.165882	31.936077
630.768365	41926.630149	31.941095
631.420153	42000.218765	31.946112
631.807894	42062.447129	31.951130
632.342240	42131.743150	31.956148
632.806829	42190.594142	31.961165
633.789409	42247.337797	31.966183
633.988994	42316.044394	31.971200
634.808623	42385.557813	31.976218
635.191852	42455.875962	31.981236
636.009163	42519.028024	31.986253
636.785404	42594.993498	31.991271
637.276058	42661.330365	31.996288
638.104807	42728.796536	32.001306
638.411585	42806.231930	32.006324
639.103577	42860.361578	32.011341
639.863926	42927.691161	32.016359
640.307753	43015.571993	32.021376
640.831642	43077.293398	32.026394
641.640145	43150.761021	32.031412
642.576953	43223.211715	32.036429
642.909265	43301.519043	32.041447
643.483442	43380.974299	32.046464
644.405995	43439.210889	32.051482
645.354531	43512.459015	32.056500
646.143180	43578.982226	32.061517
646.672951	43643.569021	32.066535
647.566760	43718.208420	32.071552
647.906056	43784.103662	32.076570
648.720650	43855.825678	32.081588
649.214182	43913.551739	32.086605
649.893520	43991.888942	32.091623
650.283913	44058.843344	32.096640
651.042119	44129.524984	32.101658
651.733106	44213.706853	32.106676
652.103958	44284.327773	32.111693
652.756467	44358.235456	32.116711
653.356937	44434.378944	32.121728
654.304157	44505.401111	32.126746
655.043128	44579.314894	32.131764
655.681770	44658.191568	32.136781
656.514655	44735.646430	32.141799
656.913501	44812.688074	32.146816
658.024888	44876.612670	32.151834
658.231495	44959.465095	32.156852
658.896345	45035.115121	32.161869
659.987512	45098.807143	32.166887
660.324360	45178.970909	32.171904
660.878604	45252.298615	32.176922
661.136293	45324.497094	32.181940
661.915138	45409.737083	32.186957
662.621928	45492.316785	32.191975
662.983340	45570.497174	32.196992
663.724942	45648.538501	32.202010
664.373723	45739.312415	32.207028
665.053426	45820.935732	32.212045
665.853463	45901.912433	32.217063
666.626319	45983.297672	32.222080
667.576408	46055.073414	32.227098
668.177765	46128.750645	32.232116
669.384343	46189.490976	32.237133
670.373292	46243.205266	32.242151
671.055910	46309.339320	32.247168
671.865760	46352.642512	32.252186
671.992205	46420.424125	32.257204
673.166604	46475.595622	32.262221
673.713493	46530.494914	32.267239
674.142731	46601.746903	32.272256
675.092736	46640.983692	32.277274
676.193284	46692.529828	32.282292
676.819705	46740.655764	32.287309
677.624570	46786.623724	32.292327
677.994134	46845.726439	32.297344
678.563891	46891.965588	32.302362
679.005812	46953.915686	32.307380
679.590933	47014.581143	32.312397
680.418886	47075.034610	32.317415
680.614387	47132.758804	32.322432
681.320527	47214.015232	32.327450
681.942270	47284.718729	32.332468
682.504432	47358.561961	32.337485
683.352400	47426.418717	32.342503
683.602316	47504.912587	32.347520
684.558933	47566.375860	32.352538
685.024861	47640.809849	32.357556
685.607726	47730.276174	32.362573
686.459184	47805.857942	32.367591
687.179409	47889.929754	32.372608
687.474599	47970.914325	32.377626
688.161784	48058.702850	32.382644
688.563760	48143.530178	32.387661
689.327688	48222.592233	32.392679
689.649122	48311.412097	32.397696
690.112125	48403.289527	32.402714
690.566493	48495.891395	32.407732
691.569452	48604.035225	32.412749
692.423704	48702.023924	32.417767
692.929350	48805.328825	32.422784
694.110905	48890.748734	32.427802
694.803757	48994.734912	32.432820
695.313860	49070.288070	32.437837
696.371889	49161.806464	32.442855
697.095145	49251.267575	32.447872
697.945130	49337.237843	32.452890
698.728300	49431.120721	32.457908
699.269130	49523.808843	32.462925
700.305271	49608.983977	32.467943
700.922160	49686.573891	32.472960
701.491703	49767.914263	32.477978
702.044352	49858.166091	32.482996
702.355549	49948.955414	32.488013
703.317248	50042.500675	32.493031
703.768055	50128.834950	32.498048
704.726993	50222.870729	32.503066
705.291985	50306.189753	32.508084
705.924796	50400.492980	32.513101
706.830329	50478.425378	32.518119
707.153024	50564.794777	32.523136
708.133175	50650.220476	32.528154
708.422556	50743.185327	32.533172
709.014213	50834.963282	32.538189
710.178106	50915.235937	32.543207
710.636409	51010.652611	32.548224
711.325800	51104.578144	32.553242
712.330717	51188.383505	32.558260
712.548688	51290.038082	32.563277
713.321521	51374.386206	32.568295
714.111231	51473.968881	32.573312
714.937165	51573.072947	32.578330
715.611953	51678.652424	32.583348
716.605831	51774.294010	32.588365
717.587367	51849.083213	32.593383
718.113634	51950.370522	32.598400
719.402479	52038.038636	32.603418
720.276764	52118.959272	32.608436
721.050289	52199.243010	32.613453
721.869888	52276.489938	32.618471
722.656503	52366.628758	32.623488
723.309990	52436.545974	32.628506
723.979770	52518.258426	32.633524
724.837460	52597.170249	32.638541
725.923104	52667.638159	32.643559
726.146675	52755.908599	32.648576
726.874853	52837.569011	32.653594
727.672853	52909.888992	32.658612
728.277822	53000.192451	32.663629
728.719455	53080.173136	32.668647
729.310338	53174.516505	32.673664
730.169213	53256.637747	32.678682
730.681209	53345.013479	32.683700
731.598350	53436.550856	32.688717
732.281870	53525.954359	32.693735
732.916446	53624.604607	32.698752
733.282744	53726.018855	32.703770
734.174826	53809.185211	32.708788
734.819418	53916.786835	32.713805
735.671098	54011.105657	32.718823
736.352311	54104.659851	32.723840
736.992761	54208.046918	32.728858
737.873798	54300.569725	32.733876
738.417922	54410.803783	32.738893
739.385342	54496.735805	32.743911
740.236620	54597.894622	32.748928
740.869423	54686.314453	32.753946
742.464805	54768.675645	32.758964
743.865266	54848.375731	32.763981
744.683583	54914.813549	32.768999
745.480704	54997.918385	32.774016
746.165345	55058.538398	32.779034
747.019654	55132.300805	32.784052
747.415409	55203.993191	32.789069
748.333701	55258.733840	32.794087
748.570181	55329.372519	32.799104
749.278913	55397.420467	32.804122
749.749530	55471.946095	32.809140
750.396768	55552.791914	32.814157
750.851637	55643.144997	32.819175
751.497641	55715.976982	32.824192
752.129331	55804.935875	32.829210
752.828055	55885.086805	32.834228
753.584477	55990.362665	32.839245
754.789295	56056.881999	32.844263
755.277987	56143.011612	32.849280
755.907741	56236.171372	32.854298
757.284822	56323.079022	32.859316
757.598630	56421.902764	32.864333
758.301334	56509.676281	32.869351
759.259223	56588.643104	32.874368
760.053179	56681.636923	32.879386
760.761067	56765.288008	32.884404
761.110739	56862.968782	32.889421
762.281366	56953.574244	32.894439
763.262753	57042.129882	32.899456
763.594691	57140.720979	32.904474
764.729382	57227.062202	32.909492
765.557261	57316.328646	32.914509
766.050851	57409.948516	32.919527
766.990016	57493.878626	32.924544
767.297229	57593.461048	32.929562
768.328303	57689.664430	32.934580
768.650128	57788.759397	32.939597
769.800185	57889.614117	32.944615
770.436991	57988.287479	32.949632
770.929919	58085.415202	32.954650
771.961500	58172.856976	32.959668
772.468115	58279.562150	32.964685
773.297480	58382.121767	32.969703
774.097939	58483.338453	32.974720
774.686967	58592.592747	32.979738
776.047803	58695.773541	32.984756
776.781328	58801.953073	32.989773
777.975802	58882.012835	32.994791
778.857886	58983.916996	32.999808
779.332090	59081.021329	33.004826
780.386621	59180.802707	33.009844
780.886208	59272.855539	33.014861
781.486707	59363.544599	33.019879
782.726578	59460.241713	33.024896
783.287286	59553.713304	33.029914
784.974173	59625.665653	33.034932
785.671994	59706.856256	33.039949
786.362481	59787.413749	33.044967
786.816316	59875.223866	33.049984
787.635679	59973.294572	33.055002
788.610583	60045.387135	33.060020
789.010492	60138.836729	33.065037
789.332854	60224.222408	33.070055
790.163818	60302.887399	33.075072
790.638667	60398.467109	33.080090
791.627414	60478.073905	33.085108
791.929650	60589.636814	33.090125
792.502223	60692.414192	33.095143
793.786340	60784.096976	33.100160
794.320127	60878.233070	33.105178
795.364189	60976.756362	33.110196
796.087295	61082.821040	33.115213
796.755314	61169.677949	33.120231
797.793428	61271.058198	33.125248
798.563210	61369.519848	33.130266
799.586284	61468.349031	33.135284
800.336108	61566.139150	33.140301
801.005231	61668.679139	33.145319
801.904335	61762.373109	33.150336
802.362190	61867.691843	33.155354
803.677140	61959.827004	33.160372
804.448517	62067.683129	33.165389
805.152329	62178.942061	33.170407
806.012414	62276.127804	33.175424
806.605941	62385.618202	33.180442
807.592576	62474.808226	33.185460
808.222575	62582.250851	33.190477
808.650099	62694.592557	33.195495
809.960849	62787.007153	33.200512
809.954481	62914.014878	33.205530
811.173166	63023.453663	33.210548
812.399382	63126.449719	33.215565
812.984567	63237.493742	33.220583
814.213800	63336.565140	33.225600
814.533924	63451.438991	33.230618
815.530453	63553.573899	33.235636
816.337129	63669.312702	33.240653
817.100835	63783.350553	33.245671
818.379882	63875.680752	33.250688
819.555684	63977.836773	33.255706
821.149183	64060.867860	33.260724
822.188931	64143.384252	33.265741
823.238246	64229.360761	33.270759
824.064447	64311.883449	33.275776
824.680630	64400.178246	33.280794
825.595484	64472.133041	33.285812
826.312003	64560.617889	33.290829
826.491299	64651.339368	33.295847
827.481063	64727.369878	33.300864
828.008352	64821.068632	33.305882
829.078697	64915.474124	33.310900
829.801149	65019.751241	33.315917
830.375846	65114.028155	33.320935
830.831089	65209.249916	33.325952
831.362500	65315.908798	33.330970
832.479493	65400.935474	33.335988
832.829923	65497.198631	33.341005
833.078130	65591.188752	33.346023
834.841732	65676.622226	33.351040
835.408602	65790.839172	33.356058
836.661443	65879.232107	33.361076
837.519873	65974.936730	33.366093
838.175610	66071.473164	33.371111
839.052609	66166.285111	33.376128
839.301504	66279.055307	33.381146
840.261396	66372.038968	33.386164
840.933612	66483.852301	33.391181
841.491258	66602.810075	33.396199
842.302270	66707.916083	33.401216
843.006680	66825.421062	33.406234
843.710904	66939.502917	33.411252
844.626684	67058.535994	33.416269
845.634963	67182.848873	33.421287
846.478665	67305.299895	33.426304
847.239447	67428.396613	33.431322
848.000576	67546.642373	33.436340
848.800295	67661.502939	33.441357
849.397753	67793.219534	33.446375
850.430613	67911.291602	33.451392
851.302074	68042.479836	33.456410
851.990825	68171.417416	33.461428
852.862983	68308.994325	33.466445
853.890644	68429.420487	33.471463
855.127888	68551.633513	33.476480
856.082646	68681.056490	33.481498
857.005075	68805.633475	33.486516
857.951825	68928.646900	33.491533
858.399448	69059.719895	33.496551
859.774291	69169.702618	33.501568
860.293413	69293.329725	33.506586
860.897338	69420.911757	33.511604
862.270707	69546.167202	33.516621
863.186663	69668.248802	33.521639
864.225862	69788.656226	33.526656
865.030377	69917.460531	33.531674
866.260544	70022.719888	33.536692
867.044610	70129.920970	33.541709
867.693760	70255.877469	33.546727
869.217995	70363.094711	33.551744
870.148835	70478.178406	33.556762
870.970256	70598.138942	33.561780
872.042287	70698.612557	33.566797
873.115909	70805.973426	33.571815
873.998720	70907.223782	33.576832
874.762960	71019.165323	33.581850
875.805952	71124.074935	33.586868
876.766433	71217.846121	33.591885
877.903744	71315.424946	33.596903
878.906950	71415.047526	33.601920
879.724790	71500.912991	33.606938
880.286687	71588.342340	33.611956
881.219235	71671.258461	33.616973
881.561131	71773.882017	33.621991
882.576400	71864.557728	33.627008
883.192299	71970.462322	33.632026
883.682366	72071.427288	33.637044
884.714962	72164.351087	33.642061
885.055781	72274.193443	33.647079
886.000867	72388.306567	33.652096
886.800796	72505.097378	33.657114
887.111424	72627.268316	33.662132
888.134725	72753.509744	33.667149
888.659180	72882.257854	33.672167
889.925048	73001.258586	33.677184
890.812429	73128.579298	33.682202
891.313098	73266.148790	33.687220
892.123888	73385.729763	33.692237
893.074610	73528.531220	33.697255
893.892291	73661.212467	33.702272
894.621911	73804.139544	33.707290
895.690195	73945.275928	33.712308
897.051243	74070.606178	33.717325
898.144500	74203.032300	33.722343
899.277124	74321.019382	33.727360
900.146243	74458.165573	33.732378
900.982475	74590.673068	33.737396
902.040740	74706.835262	33.742413
902.888634	74844.600464	33.747431
904.555437	74951.288915	33.752448
905.479222	75071.291685	33.757466
906.694725	75181.434208	33.762484
907.963111	75290.715751	33.767501
908.865876	75405.459494	33.772519
909.750295	75518.911241	33.777536
910.503114	75627.461389	33.782554
911.480727	75726.648177	33.787572
912.994525	75820.163315	33.792589
913.654365	75934.651680	33.797607
914.426545	76035.572743	33.802624
916.018947	76133.873701	33.807642
916.869716	76233.999565	33.812660
917.748276	76318.649932	33.817677
918.404519	76425.627065	33.822695
919.404330	76516.041869	33.827712
920.380162	76625.465659	33.832730
920.723228	76732.077107	33.837748
921.695737	76825.499734	33.842765
922.329597	76935.466265	33.847783
923.195247	77052.121317	33.852800
923.996743	77161.348198	33.857818
925.059415	77279.186705	33.862836
925.911847	77398.563607	33.867853
926.117063	77513.449222	33.872871
927.184095	77630.903519	33.877888
928.098486	77746.827930	33.882906
928.708727	77870.961241	33.887924
930.161810	77978.767817	33.892941
930.996838	78096.084727	33.897959
931.100213	78204.916298	33.902976
932.216643	78321.279544	33.907994
933.007653	78446.487380	33.913012
933.820918	78576.376136	33.918029
934.685182	78699.595455	33.923047
935.576013	78828.392602	33.928064
936.713605	78956.721472	33.933082
937.240294	79088.005409	33.938100
938.458525	79213.074085	33.943117
939.783400	79343.777540	33.948135
940.616706	79464.427389	33.953152
942.283519	79584.256324	33.958170
943.095947	79711.794610	33.963188
943.920013	79826.664215	33.968205
944.483134	79956.057850	33.973223
946.011866	80076.480522	33.978240
946.825069	80203.503375	33.983258
947.195874	80338.195623	33.988276
948.486379	80461.047896	33.993293
948.938081	80593.939988	33.998311
950.222313	80719.512992	34.003328
951.652177	80847.402531	34.008346
952.458117	80974.962267	34.013364
953.642546	81105.029115	34.018381
954.789168	81232.321291	34.023399
955.663971	81350.333093	34.028416
956.730717	81471.096555	34.033434
957.224505	81610.879058	34.038452
958.468866	81732.582996	34.043469
959.213745	81858.590064	34.048487
960.091074	81990.165307	34.053504
961.215934	82114.602546	34.058522
962.082393	82246.566765	34.063540
962.816081	82386.468007	34.068557
963.740236	82528.893960	34.073575
964.826463	82660.509721	34.078592
966.004330	82782.742433	34.083610
966.546755	82925.080079	34.088628
967.677549	83053.624995	34.093645
968.530138	83196.768621	34.098663
970.028293	83325.572861	34.103680
971.188535	83452.907988	34.108698
972.135594	83587.984687	34.113716
972.977282	83708.670403	34.118733
974.016601	83848.924733	34.123751
975.023783	83988.951178	34.128768
976.000424	84110.224672	34.133786
976.772347	84251.175427	34.138804
977.632073	84371.836772	34.143821
978.626263	84504.958170	34.148839
979.125039	84650.962522	34.153856
980.298789	84787.698956	34.158874
980.945969	84916.376412	34.163892
982.065797	85045.017387	34.168909
982.771269	85179.548338	34.173927
983.835309	85302.920233	34.178944
985.434058	85431.986859	34.183962
985.913693	85574.206884	34.188980
987.137479	85690.366483	34.193997
988.245781	85828.504744	34.199015
989.435957	85952.258680	34.204032
990.860548	86065.296427	34.209050
992.119562	86193.201369	34.214068
993.154164	86315.458301	34.219085
993.990209	86429.432582	34.224103
994.539891	86552.311804	34.229120
995.351375	86676.256642	34.234138
996.555511	86809.321098	34.239156
997.433644	86930.809704	34.244173
998.588707	87056.478925	34.249191
999.838116	87190.385868	34.254208
1001.201620	87321.815689	34.259226
1002.106403	87452.541507	34.264244
1002.935046	87568.533871	34.269261
1003.694309	87693.624788	34.274279
1004.731232	87823.667867	34.279296
1005.834962	87946.055879	34.284314
1006.733089	88078.247300	34.289332
1007.740570	88209.568438	34.294349
1009.064297	88334.484740	34.299367
1009.874189	88459.755428	34.304384
1010.854288	88599.765789	34.309402
1011.801420	88724.061282	34.314420
1013.001259	88852.731338	34.319437
1014.264256	88982.384961	34.324455
1015.130023	89117.851005	34.329472
1016.442491	89225.870375	34.334490
1016.914209	89369.760957	34.339508
1018.104184	89496.102837	34.344525
1019.103560	89617.542990	34.349543
1020.264161	89752.485454	34.354560
1021.320590	89871.780398	34.359578
1022.049611	90017.468327	34.364596
1023.050085	90153.406346	34.369613
1023.840064	90294.741679	34.374631
1024.721276	90429.220505	34.379648
1026.150854	90560.109234	34.384666
1027.115360	90704.119945	34.389684
1028.051915	90839.060489	34.394701
1028.925595	90972.607833	34.399719
1029.786649	91112.280122	34.404736
1030.987069	91264.510468	34.409754
1031.566608	91405.013643	34.414772
1032.367070	91553.483233	34.419789
1033.781358	91708.914522	34.424807
1034.677840	91860.033594	34.429824
1036.036476	91985.800106	34.434842
1037.449441	92133.385574	34.439860
1038.111058	92259.890681	34.444877
1038.931699	92395.826904	34.449895
1040.096143	92526.478568	34.454912
1040.800658	92665.477202	34.459930
1041.782655	92799.284025	34.464948
1042.833471	92941.625825	34.469965
1043.831967	93083.926260	34.474983
1044.356185	93229.022848	34.480000
1045.542576	93372.364186	34.485018
1046.688046	93531.861186	34.490036
1047.642355	93696.538487	34.495053
1048.585189	93843.286630	34.500071
1049.560620	93992.098936	34.505088
1050.446319	94142.387669	34.510106
1051.727004	94315.873146	34.515124
1052.829056	94476.168154	34.520141
1053.993314	94619.084566	34.525159
1055.041796	94778.144131	34.530176
1056.399945	94937.225150	34.535194
1057.689490	95078.169951	34.540212
1058.721637	95237.235370	34.545229
1060.160166	95389.879920	34.550247
1060.939189	95541.384233	34.555264
1062.049326	95688.320269	34.560282
1063.323046	95843.416894	34.565300
1064.203100	96000.557208	34.570317
1065.299911	96141.697473	34.575335
1065.869608	96304.203049	34.580352
1067.172980	96464.644677	34.585370
1068.363938	96622.486331	34.590388
1069.623484	96774.365303	34.595405
1071.156040	96928.555198	34.600423
1072.077252	97064.959229	34.605440
1073.598344	97215.490033	34.610458
1074.586035	97364.638980	34.615476
1075.545370	97510.269657	34.620493
1076.347366	97655.021621	34.625511
1077.216050	97812.802603	34.630528
1078.593073	97954.206909	34.635546
1079.421896	98118.474617	34.640564
1080.378596	98278.699494	34.645581
1081.539911	98426.480215	34.650599
1082.539313	98588.364354	34.655616
1083.714044	98741.269531	34.660634
1084.781730	98900.772520	34.665652
1085.917635	99064.802042	34.670669
1086.909026	99214.082670	34.675687
1087.572396	99379.284126	34.680704
1088.792250	99540.152923	34.685722
1090.086537	99706.679926	34.690740
1091.162633	99874.609459	34.695757
1092.302842	100032.830708	34.700775
1093.538452	100189.120770	34.705792
1094.461622	100342.665005	34.710810
1095.601452	100499.649397	34.715828
1096.407746	100652.980172	34.720845
1097.783290	100793.858037	34.725863
1098.147374	100952.569660	34.730880
1099.469663	101102.246434	34.735898
1101.038988	101248.423825	34.740916
1101.585128	101416.524742	34.745933
1102.468754	101576.138729	34.750951
1103.516537	101741.257912	34.755968
1104.746927	101898.193049	34.760986
1105.571066	102071.708789	34.766004
1106.649257	102245.362583	34.771021
1107.974787	102404.532289	34.776039
1108.701098	102581.832321	34.781056
1110.356071	102744.761219	34.786074
1111.971285	102893.554967	34.791092
1113.369462	103052.496044	34.796109
1114.943143	103215.909402	34.801127
1115.917500	103377.729656	34.806144
1116.780340	103520.635511	34.811162
1118.056218	103688.851806	34.816180
1118.748582	103850.093675	34.821197
1120.325024	104001.988680	34.826215
1121.665976	104156.004066	34.831232
1122.677726	104301.561430	34.836250
1124.489949	104442.948663	34.841268
1125.262324	104608.910141	34.846285
1126.576896	104757.706504	34.851303
1127.632924	104912.518856	34.856320
1129.147405	105051.178932	34.861338
1130.067444	105205.552847	34.866356
1130.644641	105365.272865	34.871373
1131.895734	105511.109666	34.876391
1132.763002	105674.772569	34.881408
1133.891753	105835.458551	34.886426
1135.030026	105991.036910	34.891444
1135.998782	106149.193685	34.896461
1137.062416	106320.519089	34.901479
1138.203462	106484.966720	34.906496
1139.206726	106653.519455	34.911514
1140.283434	106820.587075	34.916532
1141.231506	107001.466931	34.921549
1143.064509	107162.024484	34.926567
1144.413575	107330.799113	34.931584
1145.428838	107491.178784	34.936602
1146.656933	107651.626937	34.941620
1147.778840	107815.441131	34.946637
1148.710245	107982.590535	34.951655
1149.676261	108151.893838	34.956672
1150.889137	108318.722314	34.961690
1152.129213	108492.117389	34.966708
1152.982776	108655.688784	34.971725
1154.732682	108820.840322	34.976743
1156.120285	108983.531498	34.981760
1156.782734	109155.099016	34.986778
1158.198218	109306.597470	34.991796
1158.735149	109458.078334	34.996813
1160.101007	109613.466576	35.001831
1161.150276	109772.773533	35.006848
1162.143993	109922.595904	35.011866
1163.229942	110091.488501	35.016884
1164.035849	110252.331077	35.021901
1165.219159	110413.931231	35.026919
1165.820366	110589.664521	35.031936
1166.678267	110764.807548	35.036954
1168.382975	110948.495454	35.041972
1169.547741	111136.397714	35.046989
1170.392745	111317.477876	35.052007
1171.687003	111500.905999	35.057024
1172.774652	111682.247755	35.062042
1174.022796	111873.547941	35.067060
1174.789415	112057.431231	35.072077
1176.415252	112250.984782	35.077095
1177.744147	112437.870630	35.082112
1178.576825	112642.061610	35.087130
1180.105267	112821.334867	35.092148
1181.007199	113019.269840	35.097165
1182.391711	113205.722126	35.102183
1183.987183	113398.909585	35.107200
1185.061893	113587.002934	35.112218
1186.367661	113789.842948	35.117236
1187.277172	113975.129354	35.122253
1188.880440	114156.603343	35.127271
1189.916816	114350.729011	35.132288
1190.994340	114540.848558	35.137306
1192.393593	114734.925812	35.142324
1193.338638	114930.976052	35.147341
1194.567729	115125.418898	35.152359
1195.725784	115322.647512	35.157376
1196.911668	115519.923883	35.162394
1198.215223	115715.150792	35.167412
1199.085627	115915.778901	35.172429
1200.492825	116118.444192	35.177447
1201.824640	116310.625865	35.182464
1202.797734	116509.596192	35.187482
1204.711350	116706.417818	35.192500
1206.119909	116891.608182	35.197517
1207.758436	117064.100443	35.202535
1209.240553	117248.350970	35.207552
1210.483282	117430.450173	35.212570
1212.257272	117590.780572	35.217588
1213.697726	117761.289243	35.222605
1215.221199	117920.224254	35.227623
1216.460512	118087.734208	35.232640
1217.460418	118253.092536	35.237658
1218.716372	118417.144858	35.242676
1219.427793	118574.661727	35.247693
1220.630325	118739.009514	35.252711
1221.561684	118920.155638	35.257728
1222.542597	119098.844687	35.262746
1223.948684	119253.342538	35.267764
1224.627732	119424.584765	35.272781
1225.495314	119598.147334	35.277799
1226.662816	119767.876779	35.282816
1227.747317	119941.115865	35.287834
1228.816286	120121.146668	35.292852
1229.714131	120311.590770	35.297869
1230.574358	120496.355855	35.302887
1231.634432	120688.043352	35.307904
1232.596937	120899.720051	35.312922
1234.168608	121091.506459	35.317940
1235.032614	121297.287538	35.322957
1236.149364	121495.646326	35.327975
1237.806742	121699.784604	35.332992
1238.593793	121924.137215	35.338010
1240.101502	122135.369850	35.343028
1241.222319	122334.468868	35.348045
1242.453646	122557.325007	35.353063
1243.587648	122775.588194	35.358080
1245.291172	122985.073927	35.363098
1246.863989	123184.069446	35.368116
1248.159422	123390.583445	35.373133
1249.645411	123592.078330	35.378151
1251.399372	123791.074902	35.383168
1252.172954	124006.808892	35.388186
1253.970433	124202.622380	35.393204
1255.151559	124406.768447	35.398221
1256.757656	124606.440558	35.403239
1257.666726	124805.667631	35.408256
1258.624974	125006.750358	35.413274
1260.268438	125204.508284	35.418292
1261.215368	125416.565292	35.423309
1262.259396	125623.681067	35.428327
1263.812733	125837.012991	35.433344
1264.897211	126050.547799	35.438362
1266.418557	126256.528470	35.443380
1267.940498	126459.153753	35.448397
1269.504366	126661.609198	35.453415
1270.756969	126862.620855	35.458432
1272.323507	127072.882135	35.463450
1274.123261	127254.529531	35.468468
1275.262891	127449.216917	35.473485
1276.123051	127641.441863	35.478503
1277.217043	127840.737727	35.483520
1278.356185	128045.525808	35.488538
1279.778554	128239.059038	35.493556
1281.019417	128441.882988	35.498573
1281.656585	128660.348488	35.503591
1282.833491	128872.560360	35.508608
1284.032298	129091.345362	35.513626
1285.292275	129299.430002	35.518644
1286.262642	129520.383028	35.523661
1287.324792	129744.477763	35.528679
1289.635578	129940.770127	35.533696
1291.656718	130133.245856	35.538714
1292.858541	130323.382672	35.543732
1294.256566	130520.533675	35.548749
1295.310394	130698.356737	35.553767
1297.093416	130864.890618	35.558784
1298.330942	131050.693756	35.563802
1300.001869	131208.910989	35.568820
1301.387897	131383.999637	35.573837
1302.529716	131573.913721	35.578855
1303.834727	131742.631944	35.583872
1304.880345	131921.845031	35.588890
1305.937090	132096.635677	35.593908
1307.423248	132281.583837	35.598925
1308.577509	132460.187563	35.603943
1310.114062	132649.564640	35.608960
1310.934381	132834.242127	35.613978
1312.269290	133019.903321	35.618996
1313.684520	133208.720559	35.624013
1314.281886	133420.716708	35.629031
1316.056679	133610.695813	35.634048
1317.038020	133825.358096	35.639066
1317.781108	134024.031308	35.644084
1319.327076	134247.767970	35.649101
1320.093867	134462.722524	35.654119
1321.616888	134679.040988	35.659136
1322.875599	134905.806111	35.664154
1324.196746	135124.326761	35.669172
1325.156184	135352.410072	35.674189
1326.264051	135581.700711	35.679207
1328.510513	135800.788974	35.684224
1330.507147	135998.452823	35.689242
1332.293478	136208.582409	35.694260
1333.994591	136405.624387	35.699277
1335.051916	136613.477782	35.704295
1336.320154	136817.953718	35.709312
1337.570664	137046.206739	35.714330
1338.708230	137245.586893	35.719348
1339.940282	137452.151226	35.724365
1340.729599	137681.648321	35.729383
1342.077947	137904.608056	35.734400
1343.313184	138130.628863	35.739418
1344.512524	138352.044251	35.744436
1345.851577	138584.185577	35.749453
1346.988399	138810.911530	35.754471
1348.641937	139039.977613	35.759488
1349.578754	139271.592594	35.764506
1351.217743	139512.818068	35.769524
1352.530280	139740.524323	35.774541
1353.293424	139997.392280	35.779559
1354.930785	140224.391561	35.784576
1356.163458	140461.963241	35.789594
1357.829576	140710.063073	35.794612
1359.178616	140947.189171	35.799629
1360.537793	141194.454595	35.804647
1362.343025	141413.286839	35.809664
1363.842369	141647.669626	35.814682
1365.106232	141859.873885	35.819700
1367.307659	142066.277910	35.824717
1368.748497	142264.515223	35.829735
1369.801196	142468.062701	35.834752
1371.426813	142672.192225	35.839770
1372.584964	142878.171839	35.844788
1373.746742	143087.992672	35.849805
1374.796357	143300.633875	35.854823
1375.842807	143509.385880	35.859840
1376.960765	143748.370248	35.864858
1378.158686	143984.897477	35.869876
1379.778684	144210.763047	35.874893
1380.613210	144443.663072	35.879911
1381.701763	144678.184931	35.884928
1383.015416	144929.581744	35.889946
1384.380772	145175.990897	35.894964
1385.599470	145424.656202	35.899981
1386.935281	145675.485085	35.904999
1388.387692	145933.611373	35.910016
1389.714653	146191.062541	35.915034
1391.079008	146452.781681	35.920052
1392.750541	146703.375254	35.925069
1394.129264	146973.209123	35.930087
1395.863847	147214.099416	35.935104
1397.079866	147475.089991	35.940122
1398.858429	147728.336692	35.945140
1400.073697	147983.056671	35.950157
1401.570192	148247.355613	35.955175
1403.064816	148499.601377	35.960192
1404.448623	148757.571345	35.965210
1405.790218	149021.102625	35.970228
1407.814513	149273.270281	35.975245
1409.053564	149528.150846	35.980263
1410.419464	149790.987293	35.985280
1412.744990	150028.153725	35.990298
1414.390087	150275.762190	35.995316
1415.742370	150507.736870	36.000333
1417.010402	150756.752733	36.005351
1418.329559	150994.834109	36.010368
1419.954040	151242.719413	36.015386
1421.448332	151491.476702	36.020404
1423.077887	151721.171910	36.025421
1424.358765	151973.846246	36.030439
1425.599580	152223.219853	36.035456
1427.032079	152456.932467	36.040474
1428.480421	152692.774189	36.045492
1430.298809	152935.506621	36.050509
1431.869942	153174.337060	36.055527
1433.235327	153403.553402	36.060544
1434.650899	153639.432390	36.065562
1435.927449	153889.535492	36.070580
1437.640156	154115.392326	36.075597
1439.145059	154358.983679	36.080615
1441.602288	154567.773331	36.085632
1443.349640	154772.962063	36.090650
1444.305152	154976.845103	36.095668
1446.030260	155168.548994	36.100685
1447.542105	155369.455100	36.105703
1448.974622	155567.484067	36.110720
1449.918585	155767.798066	36.115738
1450.845289	155975.001049	36.120756
1452.192960	156184.763107	36.125773
1453.581760	156396.269733	36.130791
1454.242918	156617.276418	36.135808
1455.869714	156838.777770	36.140826
1457.033344	157078.156976	36.145844
1458.741563	157301.322138	36.150861
1459.914040	157544.126815	36.155879
1461.119896	157783.009666	36.160896
1462.317757	158022.833783	36.165914
1463.673324	158284.254784	36.170932
1465.246786	158518.367124	36.175949
1466.854247	158765.042204	36.180967
1468.313940	159012.414584	36.185984
1469.932989	159254.652997	36.191002
1471.140222	159505.289907	36.196020
1472.823250	159756.981617	36.201037
1473.852884	160017.452845	36.206055
1475.381856	160277.516939	36.211072
1476.529686	160546.114633	36.216090
1477.744806	160825.952099	36.221108
1479.629074	161085.052590	36.226125
1481.111539	161355.378632	36.231143
1482.300466	161631.447447	36.236160
1484.124818	161897.487565	36.241178
1485.409391	162170.476327	36.246196
1487.297717	162437.917968	36.251213
1488.761735	162707.737146	36.256231
1490.762332	162978.665210	36.261248
1492.506603	163234.391912	36.266266
1494.002116	163504.478337	36.271284
1496.278872	163751.423960	36.276301
1497.802302	164015.358736	36.281319
1499.208412	164260.543737	36.286336
1500.998559	164509.765883	36.291354
1502.325575	164762.272049	36.296372
1503.753398	164997.654698	36.301389
1505.800759	165250.354147	36.306407
1507.300000	165500.745303	36.311424
1509.030476	165742.908095	36.316442
1509.997967	165997.902279	36.321460
1512.018488	166243.535502	36.326477
1513.246095	166479.530092	36.331495
1514.662029	166731.261814	36.336512
1516.261554	166971.081555	36.341530
1517.583968	167225.228635	36.346548
1519.272706	167465.544696	36.351565
1520.779472	167709.772440	36.356583
1522.375464	167964.401060	36.361600
1523.843532	168200.139897	36.366618
1525.043241	168432.561552	36.371636
1526.363132	168667.045727	36.376653
1527.586330	168898.134648	36.381671
1528.528730	169141.002533	36.386688
1529.896131	169388.167857	36.391706
1531.415435	169640.359047	36.396724
1532.758936	169889.573579	36.401741
1534.471341	170150.350219	36.406759
1535.965467	170402.829438	36.411776
1537.647812	170661.939908	36.416794
1538.639599	170925.918628	36.421812
1540.444245	171191.406358	36.426829
1542.125796	171451.816056	36.431847
1543.008711	171732.117777	36.436864
1544.980787	172003.470298	36.441882
1546.424201	172283.217541	36.446900
1547.945953	172545.714864	36.451917
1549.427597	172825.459858	36.456935
1550.964218	173095.975675	36.461952
1552.735289	173372.798908	36.466970
1554.140066	173657.103402	36.471988
1555.683025	173942.377452	36.477005
1557.490645	174222.422939	36.482023
1558.768141	174513.616781	36.487040
1560.725331	174787.388219	36.492058
1562.040647	175089.782014	36.497076
1563.514399	175359.358850	36.502093
1565.547633	175654.931756	36.507111
1566.977004	175931.458855	36.512128
1568.766539	176222.989528	36.517146
1570.192364	176505.572529	36.522164
1571.898956	176797.767456	36.527181
1573.579250	177079.438572	36.532199
1574.992496	177371.214720	36.537216
1576.365157	177648.586947	36.542234
1578.340484	177948.841560	36.547252
1580.171065	178231.346609	36.552269
1581.532284	178523.659223	36.557287
1582.529800	178821.258811	36.562304
1584.602188	179104.682849	36.567322
1585.968095	179397.444811	36.572340
1587.918022	179697.842763	36.577357
1589.404803	179999.838915	36.582375
1590.924344	180292.062409	36.587392
1592.392391	180573.333764	36.592410
1594.178054	180875.060210	36.597428
1595.931420	181165.387355	36.602445
1597.527644	181457.327418	36.607463
1599.239129	181752.055221	36.612480
1601.241423	182023.240137	36.617498
1603.181074	182309.091732	36.622516
1604.991613	182590.803887	36.627533
1607.207671	182873.760354	36.632551
1608.517124	183147.270049	36.637568
1610.150795	183410.743951	36.642586
1611.708255	183662.735515	36.647604
1613.896124	183885.253782	36.652621
1615.772216	184119.559884	36.657639
1617.353432	184366.793321	36.662656
1618.738031	184609.415169	36.667674
1620.302740	184847.479716	36.672692
1621.818568	185083.687978	36.677709
1623.533576	185316.338239	36.682727
1625.419331	185561.131590	36.687744
1627.171138	185784.172620	36.692762
1628.614164	186033.074032	36.697780
1630.219387	186280.301406	36.702797
1631.344728	186512.531148	36.707815
1632.661104	186771.608314	36.712832
1634.364434	187021.565045	36.717850
1636.032764	187292.834779	36.722868
1637.529533	187563.828789	36.727885
1639.483414	187803.483870	36.732903
1641.159613	188073.525984	36.737920
1642.746507	188323.876210	36.742938
1644.381112	188582.291099	36.747956
1645.828206	188839.049391	36.752973
1647.631217	189103.887000	36.757991
1648.924059	189375.241100	36.763008
1650.661806	189639.406783	36.768026
1652.000079	189922.305037	36.773044
1653.129025	190198.588363	36.778061
1655.053603	190469.328035	36.783079
1656.647366	190751.898715	36.788096
1658.560284	191036.653936	36.793114
1659.823399	191320.232248	36.798132
1661.379602	191603.143813	36.803149
1663.217516	191890.187611	36.808167
1664.419172	192181.027227	36.813184
1666.170873	192482.936713	36.818202
1668.081570	192781.878437	36.823220
1669.710444	193072.553931	36.828237
1671.955487	193354.503155	36.833255
1674.218079	193636.705017	36.838272
1675.824684	193918.898418	36.843290
1677.728207	194201.541225	36.848308
1679.164011	194486.620536	36.853325
1680.921888	194763.933749	36.858343
1682.304976	195051.715250	36.863360
1683.974875	195334.096870	36.868378
1685.859421	195627.627547	36.873396
1687.307342	195909.451068	36.878413
1689.058747	196192.395608	36.883431
1690.697871	196494.143882	36.888448
1692.346295	196776.854125	36.893466
1693.816969	197070.420638	36.898484
1695.661270	197369.729871	36.903501
1697.632562	197651.086262	36.908519
1699.413027	197947.540437	36.913536
1700.763913	198220.291334	36.918554
1702.930874	198495.592191	36.923572
1704.074797	198774.255475	36.928589
1705.933801	199032.219030	36.933607
1707.549656	199309.782051	36.938624
1708.786250	199579.549836	36.943642
1710.662654	199860.476010	36.948660
1712.558544	200130.611494	36.953677
1714.437056	200406.564503	36.958695
1715.794777	200697.884130	36.963712
1717.234967	200973.922290	36.968730
1719.302686	201239.301404	36.973748
1721.664589	201511.933742	36.978765
1723.505326	201784.904041	36.983783
1725.202417	202060.614884	36.988800
1726.779837	202333.261568	36.993818
1728.603370	202615.593774	36.998836
1730.099619	202899.769164	37.003853
1731.998328	203181.051386	37.008871
1733.197461	203478.694095	37.013888
1734.746733	203766.115007	37.018906
1736.876634	204058.611587	37.023924
1737.940322	204359.047646	37.028941
1739.669844	204655.101666	37.033959
1741.176455	204969.903678	37.038976
1743.085056	205271.987492	37.043994
1744.970037	205571.271195	37.049012
1746.483610	205881.240511	37.054029
1748.657396	206199.789574	37.059047
1749.945698	206514.025195	37.064064
1751.620091	206833.431306	37.069082
1753.586759	207133.788966	37.074100
1754.781840	207467.835212	37.079117
1756.742649	207802.701140	37.084135
1758.201102	208135.972965	37.089152
1759.732922	208464.055471	37.094170
1761.837740	208800.224278	37.099188
1763.736825	209135.932479	37.104205
1765.767107	209456.133726	37.109223
1767.589305	209781.917418	37.114240
1769.629561	210111.413264	37.119258
1771.546766	210432.323004	37.124276
1773.170490	210766.649119	37.129293
1775.243079	211095.294382	37.134311
1776.999482	211419.395789	37.139328
1778.763836	211730.243476	37.144346
1780.625561	212058.152727	37.149364
1782.006400	212394.798394	37.154381
1784.186526	212712.211903	37.159399
1786.094895	213041.261312	37.164416
1787.874109	213364.086531	37.169434
1789.643553	213689.289004	37.174452
1791.375823	214020.364491	37.179469
1793.365631	214348.379085	37.184487
1795.200569	214666.110668	37.189504
1797.016082	214980.901329	37.194522
1798.636111	215295.191242	37.199540
1800.183981	215595.413937	37.204557
1802.349305	215887.134987	37.209575
1804.225989	216192.323121	37.214592
1806.062692	216488.936183	37.219610
1808.447754	216775.179338	37.224628
1810.110495	217063.023820	37.229645
1812.044038	217362.672372	37.234663
1813.937870	217643.981906	37.239680
1816.371594	217925.308426	37.244698
1818.931226	218197.995009	37.249716
1820.251497	218472.491853	37.254733
1822.267006	218749.202893	37.259751
1823.798109	219036.644538	37.264768
1825.523924	219335.242375	37.269786
1827.458951	219599.348706	37.274804
1829.241944	219887.464736	37.279821
1831.115013	220173.828095	37.284839
1832.582368	220474.477701	37.289856
1834.198400	220758.154229	37.294874
1836.042283	221052.067687	37.299892
1837.310454	221360.904050	37.304909
1839.097843	221660.669567	37.309927
1840.946961	221978.570964	37.314944
1841.940455	222350.090942	37.319962
1844.144928	222672.179724	37.324980
1845.861571	223001.343598	37.329997
1847.866110	223328.380757	37.335015
1849.507753	223651.527913	37.340032
1851.556906	223970.307192	37.345050
1853.605762	224292.084452	37.350068
1855.237289	224634.423440	37.355085
1857.506131	224958.517529	37.360103
1859.729738	225271.382472	37.365120
1861.400184	225594.177295	37.370138
1863.870536	225903.145311	37.375156
1865.844038	226223.405685	37.380173
1867.999652	226545.339923	37.385191
1869.773815	226850.879183	37.390208
1872.048390	227162.333651	37.395226
1874.130949	227461.019947	37.400244
1875.726247	227772.609848	37.405261
1877.753108	228075.319763	37.410279
1879.767590	228377.499367	37.415296
1881.461101	228690.727755	37.420314
1883.574806	228991.750874	37.425332
1885.449106	229301.244794	37.430349
1887.579950	229600.108513	37.435367
1889.423803	229897.190184	37.440384
1891.121542	230199.858005	37.445402
1893.348653	230503.357119	37.450420
1895.011555	230806.489630	37.455437
1896.850837	231106.928414	37.460455
1899.077061	231396.335030	37.465472
1900.414676	231692.105982	37.470490
1902.808566	231965.893625	37.475508
1904.565073	232242.196001	37.480525
1906.925968	232499.964447	37.485543
1909.120991	232757.683717	37.490560
1910.780188	233016.225254	37.495578
1912.955106	233283.295561	37.500596
1914.621570	233553.368071	37.505613
1916.266393	233811.964791	37.510631
1918.523991	234076.204937	37.515648
1920.203201	234348.919010	37.520666
1922.149737	234618.467403	37.525684
1923.886674	234885.535334	37.530701
1925.686014	235157.927747	37.535719
1927.614078	235438.123214	37.540736
1929.137616	235731.616327	37.545754
1931.125780	236012.565772	37.550772
1932.680982	236304.328359	37.555789
1933.946131	236603.147864	37.560807
1936.381853	236910.011698	37.565824
1937.908538	237221.998869	37.570842
1939.939697	237523.518671	37.575860
1941.898785	237829.444795	37.580877
1943.710177	238142.024401	37.585895
1945.561969	238460.211719	37.590912
1947.575490	238783.657345	37.595930
1949.650899	239095.765937	37.600948
1951.390835	239420.679166	37.605965
1953.284527	239746.711897	37.610983
1955.741780	240052.742808	37.616000
1957.539264	240383.593122	37.621018
1959.600789	240693.904853	37.626036
1961.896480	241028.335481	37.631053
1964.265493	241351.604847	37.636071
1966.263500	241659.084365	37.641088
1967.729428	241982.574907	37.646106
1969.703802	242300.981796	37.651124
1971.768914	242625.521940	37.656141
1973.611707	242955.508447	37.661159
1975.656537	243267.810544	37.666176
1977.580535	243594.077370	37.671194
1979.895966	243926.582211	37.676212
1981.893740	244254.159803	37.681229
1983.929186	244585.262902	37.686247
1985.570773	244910.129961	37.691264
1987.231095	245243.478650	37.696282
1989.084612	245574.435226	37.701300
1991.020037	245913.685656	37.706317
1993.158368	246247.087916	37.711335
1995.817356	246562.703913	37.716352
1998.162264	246899.148433	37.721370
2000.643711	247217.334132	37.726388
2002.714564	247535.230053	37.731405
2004.923352	247845.230419	37.736423
2007.050173	248154.609401	37.741440
2009.056534	248455.498712	37.746458
2011.183906	248737.928083	37.751476
2013.139954	249028.361167	37.756493
2014.709166	249314.893549	37.761511
2016.997160	249594.504828	37.766528
2018.631187	249883.441081	37.771546
2020.317704	250162.818555	37.776564
2022.437341	250458.511786	37.781581
2024.237218	250756.669428	37.786599
2026.432308	251051.792904	37.791616
2028.393336	251361.280577	37.796634
2030.330077	251657.030322	37.801652
2032.345397	251960.541044	37.806669
2034.268494	252273.313179	37.811687
2036.212392	252571.476490	37.816704
2037.691944	252889.400432	37.821722
2039.719699	253206.729910	37.826740
2041.731335	253531.048031	37.831757
2044.007051	253856.874335	37.836775
2046.347916	254170.243837	37.841792
2048.349592	254502.947858	37.846810
2050.328130	254820.795844	37.851828
2052.685359	255137.034719	37.856845
2054.425512	255472.652273	37.861863
2056.390446	255791.901042	37.866880
2058.173733	256127.207969	37.871898
2060.117778	256468.205442	37.876916
2062.249300	256803.153334	37.881933
2064.242768	257153.695319	37.886951
2066.366368	257488.264446	37.891968
2068.311494	257842.193673	37.896986
2070.853335	258179.085271	37.902004
2072.825848	258532.858756	37.907021
2074.420544	258883.796783	37.912039
2076.549278	259231.475249	37.917056
2078.562437	259595.023790	37.922074
2080.555460	259955.400684	37.927092
2083.068833	260309.573451	37.932109
2085.222093	260671.551643	37.937127
2087.106656	261022.751320	37.942144
2089.196619	261388.906515	37.947162
2091.130556	261750.361973	37.952180
2093.738445	262122.227751	37.957197
2095.570458	262483.903448	37.962215
2097.668033	262843.124140	37.967232
2099.550099	263210.279731	37.972250
2101.758204	263582.083552	37.977268
2104.146217	263940.039968	37.982285
2106.791736	264294.678892	37.987303
2109.460489	264635.444377	37.992320
2111.910596	264984.526253	37.997338
2113.971735	265333.771738	38.002356
2116.420017	265672.007348	38.007373
2118.269166	266012.624538	38.012391
2120.773168	266357.177220	38.017408
2122.990649	266675.991349	38.022426
2124.653796	266987.374257	38.027444
2126.398623	267295.645206	38.032461
2128.386628	267614.216886	38.037479
2130.567665	267931.589582	38.042496
2132.652112	268252.254797	38.047514
2134.438104	268584.576823	38.052532
2136.589547	268898.830118	38.057549
2138.423637	269237.114624	38.062567
2140.735336	269549.285131	38.067584
2142.722100	269882.592074	38.072602
2144.724354	270224.356014	38.077620
2146.684131	270566.152232	38.082637
2148.746564	270903.715336	38.087655
2150.760672	271248.297550	38.092672
2152.861095	271608.413054	38.097690
2154.982897	271958.694163	38.102708
2157.073537	272308.116591	38.107725
2159.094019	272680.133849	38.112743
2161.156805	273031.237474	38.117760
2163.413685	273407.739189	38.122778
2165.332838	273779.671100	38.127796
2167.604106	274141.995524	38.132813
2169.982849	274512.203394	38.137831
2172.086912	274881.692741	38.142848
2174.413553	275253.458504	38.147866
2177.122235	275633.470587	38.152884
2179.367562	275997.297948	38.157901
2181.705925	276364.641596	38.162919
2184.127301	276733.191398	38.167936
2186.531369	277088.026052	38.172954
2188.501031	277459.644967	38.177972
2190.756710	277837.493079	38.182989
2192.953554	278203.258411	38.188007
2194.987045	278573.368117	38.193024
2197.302440	278938.453939	38.198042
2199.276262	279319.674125	38.203060
2201.866305	279687.688309	38.208077
2204.079744	280058.632637	38.213095
2206.171268	280434.270339	38.218112
2208.463362	280803.093364	38.223130
2210.277539	281180.730716	38.228148
2212.953403	281557.265884	38.233165
2214.774427	281939.017035	38.238183
2217.170137	282319.940113	38.243200
2219.459664	282700.473316	38.248218
2221.285783	283089.666016	38.253236
2223.785859	283462.747535	38.258253
2225.604508	283857.732740	38.263271
2227.887632	284242.584308	38.268288
2230.085869	284637.915089	38.273306
2232.439600	285039.749440	38.278324
2235.121669	285409.498054	38.283341
2236.947892	285801.406473	38.288359
2239.200557	286183.949360	38.293376
2241.654034	286560.642717	38.298394
2243.449816	286936.906498	38.303412
2245.821039	287291.994180	38.308429
2247.903832	287658.202886	38.313447
2249.961637	288024.796183	38.318464
2252.353556	288387.500242	38.323482
2254.071278	288752.800247	38.328500
2256.906248	289109.285704	38.333517
2258.940488	289481.164743	38.338535
2261.590748	289846.188493	38.343552
2264.261584	290218.905511	38.348570
2266.443463	290582.478375	38.353588
2269.115122	290930.960129	38.358605
2271.583455	291297.941328	38.363623
2274.019579	291658.119214	38.368640
2276.722124	291998.211748	38.373658
2279.312521	292351.276845	38.378676
2281.493341	292698.716205	38.383693
2283.896145	293062.123357	38.388711
2285.877361	293416.172492	38.393728
2288.317043	293765.753773	38.398746
2290.341675	294120.455350	38.403764
2292.839677	294473.785773	38.408781
2295.053249	294842.046377	38.413799
2297.138702	295204.255523	38.418816
2299.087954	295567.019056	38.423834
2301.375235	295934.529322	38.428852
2303.783846	296305.372724	38.433869
2305.263131	296700.164365	38.438887
2307.869394	297079.535374	38.443904
2310.339822	297463.296256	38.448922
2312.316679	297844.010156	38.453940
2315.027142	298226.562876	38.458957
2317.567328	298608.735332	38.463975
2319.357095	299006.495495	38.468992
2322.093310	299395.950784	38.474010
2324.004760	299797.830242	38.479028
2326.403170	300180.428036	38.484045
2328.770244	300582.411144	38.489063
2330.778351	300986.964874	38.494080
2333.633507	301390.621245	38.499098
2335.233492	301795.898005	38.504116
2337.695701	302204.847168	38.509133
2339.856533	302611.074279	38.514151
2342.196413	303021.488450	38.519168
2344.757729	303444.490606	38.524186
2346.747112	303867.810785	38.529204
2349.375894	304269.488511	38.534221
2351.727225	304687.871898	38.539239
2354.112649	305104.749973	38.544256
2356.744203	305509.979717	38.549274
2359.064894	305933.063214	38.554292
2361.613381	306338.481401	38.559309
2364.411315	306747.287822	38.564327
2366.807419	307153.997622	38.569344
2369.500867	307549.127337	38.574362
2371.907528	307917.453430	38.579380
2374.227138	308289.399022	38.584397
2376.708002	308670.030085	38.589415
2378.669750	309025.215435	38.594432
2381.287197	309386.874330	38.599450
2383.432775	309761.052745	38.604468
2385.879505	310134.826639	38.609485
2388.306656	310498.264843	38.614503
2390.482686	310891.611399	38.619520
2392.926136	311261.800832	38.624538
2395.011633	311657.191020	38.629556
2397.120191	312033.349001	38.634573
2399.569918	312428.043728	38.639591
2401.769307	312832.021923	38.644608
2404.591435	313213.066326	38.649626
2406.472394	313621.206636	38.654644
2409.237416	314013.788257	38.659661
2411.440633	314416.616876	38.664679
2413.478683	314827.394429	38.669696
2416.017650	315232.046131	38.674714
2418.864095	315646.882987	38.679732
2421.165266	316061.271188	38.684749
2423.693009	316468.764277	38.689767
2426.010877	316890.562588	38.694784
2428.746082	317308.940414	38.699802
2431.184772	317728.836487	38.704820
2433.308265	318142.202687	38.709837
2436.033646	318577.592910	38.714855
2438.055516	319006.006736	38.719872
2440.883770	319425.376344	38.724890
2442.857534	319857.273265	38.729908
2445.952718	320279.542718	38.734925
2448.499219	320710.760667	38.739943
2450.915184	321139.381351	38.744960
2453.674830	321557.278895	38.749978
2456.665122	321976.001377	38.754996
2459.673647	322385.373069	38.760013
2462.390064	322786.992442	38.765031
2464.610159	323206.440508	38.770048
2467.644071	323606.456528	38.775066
2469.977600	324013.946452	38.780084
2472.169468	324410.587426	38.785101
2474.867683	324810.752440	38.790119
2477.078255	325216.782962	38.795136
2479.738317	325611.007535	38.800154
2482.365117	326013.107996	38.805172
2484.573796	326424.719699	38.810189
2487.448239	326828.351301	38.815207
2489.983364	327236.758057	38.820224
2492.253505	327636.291099	38.825242
2494.719289	328050.900894	38.830260
2497.020728	328450.145422	38.835277
2499.423264	328867.985919	38.840295
2501.388093	329289.829575	38.845312
2504.226214	329686.417724	38.850330
2506.460263	330073.983051	38.855348
2508.743560	330448.409933	38.860365
2511.389584	330820.441213	38.865383
2513.464501	331211.784028	38.870400
2515.927303	331590.823634	38.875418
2518.100652	331987.326915	38.880436
2520.401297	332389.699040	38.885453
2523.531544	332788.712524	38.890471
2525.492009	333193.952605	38.895488
2527.912865	333599.929961	38.900506
2530.275919	334015.207786	38.905524
2532.205126	334437.890263	38.910541
2534.832936	334857.082276	38.915559
2537.257114	335300.934302	38.920576
2539.758174	335734.309762	38.925594
2542.041863	336181.174496	38.930612
2544.561282	336632.645543	38.935629
2547.059693	337077.159592	38.940647
2549.517528	337541.228311	38.945664
2551.913931	337992.506371	38.950682
2554.648637	338457.261019	38.955700
2557.076535	338926.174206	38.960717
2560.121192	339392.320227	38.965735
2562.610104	339859.236403	38.970752
2565.237171	340325.060837	38.975770
2567.613804	340796.735765	38.980788
2570.411727	341266.563075	38.985805
2573.227993	341728.132289	38.990823
2575.556766	342214.250580	38.995840
2578.367806	342686.426099	39.000858
2580.783648	343166.810376	39.005876
2583.385297	343639.138516	39.010893
2586.548212	344115.842364	39.015911
2589.069924	344594.091075	39.020928
2592.095630	345066.949919	39.025946
2595.081538	345538.135622	39.030964
2597.839200	346005.951689	39.035981
2601.052302	346461.734278	39.040999
2603.149619	346942.518761	39.046016
2605.530860	347397.689394	39.051034
2608.744708	347854.526918	39.056052
2611.160452	348325.322878	39.061069
2614.340867	348784.112855	39.066087
2616.424803	349241.625700	39.071104
2619.364104	349705.294969	39.076122
2622.240115	350164.603962	39.081140
2624.590084	350615.665916	39.086157
2627.417693	351071.344730	39.091175
2630.394169	351523.619858	39.096192
2633.035590	351981.833529	39.101210
2635.886074	352420.083095	39.106228
2638.249261	352874.728454	39.111245
2640.995339	353322.049300	39.116263
2643.326960	353772.604961	39.121280
2645.669741	354221.378060	39.126298
2648.223280	354658.919670	39.131316
2650.270666	355082.373754	39.136333
2653.325210	355496.247604	39.141351
2655.846830	355931.574984	39.146368
2658.258250	356357.651334	39.151386
2661.057294	356791.277436	39.156404
2663.402105	357229.337474	39.161421
2666.157982	357656.388831	39.166439
2668.652837	358096.904861	39.171456
2671.645924	358539.317789	39.176474
2674.277424	358988.814633	39.181492
2676.607476	359438.329677	39.186509
2679.160690	359881.104609	39.191527
2681.958723	360341.450910	39.196544
2684.222123	360803.070330	39.201562
2686.877887	361265.790609	39.206580
2689.420098	361746.899444	39.211597
2691.721459	362217.737330	39.216615
2694.765943	362706.751363	39.221632
2697.281009	363199.118010	39.226650
2699.998857	363683.681343	39.231668
2702.430094	364178.334899	39.236685
2705.135731	364665.884452	39.241703
2707.623611	365166.507600	39.246720
2710.189665	365681.197500	39.251738
2712.916638	366184.385381	39.256756
2715.427432	366715.186869	39.261773
2718.104023	367229.613021	39.266791
2720.848489	367761.177023	39.271808
2723.421174	368281.317079	39.276826
2726.444798	368825.106084	39.281844
2729.086900	369355.753341	39.286861
2732.283958	369873.009491	39.291879
2734.710316	370413.092140	39.296896
2737.720452	370946.985569	39.301914
2741.163933	371472.277847	39.306932
2743.769130	372010.992368	39.311949
2746.717182	372531.934782	39.316967
2749.575771	373061.714825	39.321984
2752.473906	373593.207219	39.327002
2755.117230	374112.198951	39.332020
2757.739805	374649.531722	39.337037
2760.836203	375168.489068	39.342055
2763.793039	375693.703357	39.347072
2766.747150	376218.759024	39.352090
2769.919954	376732.178578	39.357108
2772.622374	377253.886182	39.362125
2775.796331	377762.649429	39.367143
2778.916655	378273.672578	39.372160
2781.482205	378780.134261	39.377178
2784.691057	379288.491732	39.382196
2787.236833	379798.723417	39.387213
2790.325708	380297.547885	39.392231
2792.851148	380800.463358	39.397248
2795.827841	381292.367102	39.402266
2798.975833	381759.097809	39.407284
2802.129153	382206.567942	39.412301
2804.904000	382643.489185	39.417319
2807.773124	383082.749583	39.422336
2810.658085	383516.954366	39.427354
2813.603340	383957.892046	39.432372
2816.216758	384421.199247	39.437389
2819.177532	384850.125732	39.442407
2821.714909	385288.119047	39.447424
2823.764697	385748.226730	39.452442
2827.023614	386194.313345	39.457460
2829.730474	386653.417862	39.462477
2832.110406	387124.870016	39.467495
2834.724534	387600.261100	39.472512
2836.922744	388083.346214	39.477530
2839.644492	388568.599280	39.482548
2841.841658	389065.342122	39.487565
2844.663225	389568.522720	39.492583
2847.279942	390081.239427	39.497600
2849.851010	390612.317851	39.502618
2852.638030	391136.709384	39.507636
2855.410948	391667.486270	39.512653
2857.941000	392215.107612	39.517671
2860.696256	392759.007426	39.522688
2863.804481	393303.552868	39.527706
2866.551436	393847.665045	39.532724
2868.905459	394411.636151	39.537741
2871.965226	394980.278960	39.542759
2874.516828	395541.030215	39.547776
2877.198601	396130.862195	39.552794
2880.527474	396702.450928	39.557812
2883.333253	397290.619980	39.562829
2886.460454	397861.967177	39.567847
2889.592247	398446.590292	39.572864
2891.972630	399026.631209	39.577882
2895.691626	399607.945906	39.582900
2898.781732	400197.640741	39.587917
2901.849963	400785.401412	39.592935
2904.942650	401359.481894	39.597952
2907.779052	401946.117182	39.602970
2910.838210	402524.086526	39.607988
2913.696161	403110.342078	39.613005
2916.880837	403685.050705	39.618023
2919.903685	404262.436378	39.623040
2922.773183	404850.381684	39.628058
2925.831952	405423.227841	39.633076
2928.682439	406010.647296	39.638093
2932.003314	406573.214742	39.643111
2935.604278	407147.844426	39.648128
2938.199786	407713.294252	39.653146
2941.690923	408274.789662	39.658164
2944.858378	408843.372587	39.663181
2947.891628	409401.649821	39.668199
2950.696896	409947.710385	39.673216
2953.905871	410484.547161	39.678234
2957.096078	411007.817306	39.683252
2959.664306	411514.068620	39.688269
2962.607156	412019.973231	39.693287
2965.633357	412522.941397	39.698304
2968.095324	413042.692017	39.703322
2970.932399	413555.100474	39.708340
2973.901316	414069.709301	39.713357
2976.518287	414588.799728	39.718375
2979.404592	415121.244305	39.723392
2982.442116	415647.927924	39.728410
2985.668337	416174.343995	39.733428
2988.642108	416702.260148	39.738445
2991.407625	417233.240373	39.743463
2994.658793	417766.237070	39.748480
2997.412357	418317.420199	39.753498
3000.477929	418858.255624	39.758516
3003.391452	419398.116542	39.763533
3006.232655	419949.532634	39.768551
3009.061357	420501.750641	39.773568
3012.238900	421065.228113	39.778586
3015.074542	421629.787053	39.783604
3017.783258	422189.236710	39.788621
3020.504818	422762.658105	39.793639
3023.970381	423337.469877	39.798656
3026.364988	423928.374310	39.803674
3029.561635	424520.836366	39.808692
3032.662794	425110.260613	39.813709
3035.583714	425706.768324	39.818727
3038.768719	426298.990571	39.823744
3041.561119	426897.924043	39.828762
3044.530012	427505.124695	39.833780
3047.781729	428120.575079	39.838797
3050.893789	428729.422194	39.843815
3054.332432	429323.664635	39.848832
3057.117438	429953.229124	39.853850
3060.071857	430568.466687	39.858868
3063.062249	431179.023798	39.863885
3066.519340	431795.545801	39.868903
3070.186351	432408.170307	39.873920
3072.920679	433026.347484	39.878938
3076.422014	433624.710906	39.883956
3079.537515	434242.671775	39.888973
3082.396107	434862.329657	39.893991
3086.066435	435469.384978	39.899008
3089.258296	436080.907526	39.904026
3092.261440	436674.491829	39.909044
3095.577914	437274.317507	39.914061
3098.843356	437881.733060	39.919079
3102.232078	438483.771735	39.924096
3104.929953	439089.677686	39.929114
3108.440884	439687.464694	39.934132
3111.311760	440290.807175	39.939149
3113.835873	440887.100732	39.944167
3117.417213	441502.605276	39.949184
3119.917425	442093.759064	39.954202
3122.863709	442674.549671	39.959220
3125.946436	443246.393794	39.964237
3128.683377	443827.291012	39.969255
3131.501524	444408.009431	39.974272
3134.340039	445000.152132	39.979290
3137.477281	445583.019039	39.984308
3140.249688	446181.724065	39.989325
3142.901966	446799.467102	39.994343
3146.215195	447402.510410	39.999360
3148.973412	448024.912300	40.004378
3152.158452	448647.381967	40.009396
3155.540687	449273.448267	40.014413
3158.108628	449909.294164	40.019431
3161.391531	450539.391266	40.024448
3164.275978	451196.511021	40.029466
3167.369117	451839.812567	40.034484
3170.203760	452505.860950	40.039501
3173.181596	453183.659072	40.044519
3176.453333	453852.078731	40.049536
3179.542363	454541.761963	40.054554
3182.993732	455219.171153	40.059572
3186.315308	455901.286477	40.064589
3189.635042	456595.778558	40.069607
3193.010972	457273.289243	40.074624
3196.003815	457967.638372	40.079642
3199.381360	458665.648970	40.084660
3202.647944	459359.961569	40.089677
3205.727479	460059.391684	40.094695
3209.301824	460760.744805	40.099712
3212.530091	461459.347614	40.104730
3215.635034	462162.247423	40.109748
3219.036317	462869.225586	40.114765
3222.236779	463582.636568	40.119783
3225.562241	464298.937859	40.124800
3228.958854	465023.499234	40.129818
3232.155281	465733.348856	40.134836
3235.786111	466447.961487	40.139853
3238.934266	467161.918188	40.144871
3242.475007	467872.197750	40.149888
3245.600747	468585.098080	40.154906
3248.968278	469302.284940	40.159924
3252.563792	469999.334901	40.164941
3255.773060	470707.699111	40.169959
3259.473761	471404.482780	40.174976
3262.702081	472111.986621	40.179994
3266.171739	472818.214356	40.185012
3269.714886	473510.299545	40.190029
3272.679534	474211.856670	40.195047
3275.958570	474924.361298	40.200064
3279.290022	475631.321933	40.205082
3282.694481	476322.978920	40.210100
3286.119447	477028.460070	40.215117
3289.266565	477729.612916	40.220135
3293.160082	478411.869522	40.225152
3296.047185	479096.283680	40.230170
3299.352659	479750.786374	40.235188
3302.754495	480398.731980	40.240205
3305.599243	481054.376110	40.245223
3308.857640	481692.344911	40.250240
3312.234852	482349.630291	40.255258
3314.935849	482999.622025	40.260276
3318.057562	483664.130064	40.265293
3321.175505	484345.190752	40.270311
3324.024790	485017.325773	40.275328
3327.084138	485702.289113	40.280346
3329.824260	486405.114728	40.285364
3333.217697	487091.036521	40.290381
3336.015734	487821.084709	40.295399
3339.596062	488529.913341	40.300416
3342.780757	489247.517905	40.305434
3345.940485	489979.749335	40.310452
3349.271532	490716.117922	40.315469
3352.670191	491468.106202	40.320487
3355.847338	492202.722923	40.325504
3359.302260	492965.602840	40.330522
3362.504482	493724.299048	40.335540
3366.140879	494474.864897	40.340557
3369.411023	495246.972614	40.345575
3372.506918	496020.236816	40.350592
3376.504349	496777.367781	40.355610
3379.620381	497565.813962	40.360628
3383.349799	498335.799017	40.365645
3386.690136	499115.810326	40.370663
3390.111454	499894.058262	40.375680
3393.449646	500674.456509	40.380698
3397.017519	501472.858446	40.385716
3400.734197	502238.992046	40.390733
3404.369905	503042.815361	40.395751
3407.838923	503823.054380	40.400768
3411.414317	504604.402932	40.405786
3415.024754	505385.812040	40.410804
3418.710098	506155.464592	40.415821
3422.083840	506951.982776	40.420839
3425.657268	507727.488407	40.425856
3429.318369	508517.328212	40.430874
3432.505364	509288.080933	40.435892
3436.254400	510068.045571	40.440909
3439.648065	510849.645497	40.445927
3442.983089	511628.746450	40.450944
3446.545141	512424.324878	40.455962
3449.616905	513194.313669	40.460980
3453.347636	513986.411566	40.465997
3456.516738	514784.311926	40.471015
3459.909720	515567.509808	40.476032
3463.388621	516363.621153	40.481050
3466.814110	517161.922219	40.486068
3470.196855	517957.921902	40.491085
3473.622244	518758.566997	40.496103
3477.100046	519562.947357	40.501120
3480.766372	520335.141198	40.506125
3483.801122	521086.263045	40.511130
3487.115791	521767.135667	40.516135
3490.118821	522419.112679	40.521140
3493.296860	522985.452613	40.526144
3495.682614	523508.121951	40.531149
3498.475315	523965.199607	40.536154
3501.170453	524374.310684	40.541159
3503.434324	524731.568988	40.546164
3505.215089	525011.056601	40.551168
3507.110630	525251.804365	40.556173
3508.632148	525454.851607	40.561178
3510.466774	525614.228158	40.566183
3511.834810	525731.827551	40.571188
3513.017306	525796.689109	40.576192
3514.289135	525833.182025	40.581197
3515.074144	525842.054606	40.586202
3516.100601	525809.494794	40.591207
3516.871912	525767.928119	40.596212
3517.529669	525693.021047	40.601216
3518.312266	525595.753842	40.606221
3518.811713	525477.150907	40.611226
3519.691597	525338.825382	40.616231
3519.816263	525188.335737	40.621236
3520.157694	525015.772831	40.626240
3520.146355	524820.063421	40.631245
3520.102752	524635.577979	40.636250
3520.435123	524422.623704	40.641255
3520.965283	524222.676602	40.646260
3520.967434	524003.046160	40.651264
3521.082742	523766.410423	40.656269
3520.992268	523537.740032	40.661274
3520.839960	523300.533171	40.666279
3520.837101	523053.997808	40.671284
3520.786907	522813.987364	40.676288
3520.583986	522561.056030	40.681293
3520.475032	522316.396663	40.686298
3520.598792	522067.905266	40.691303
3520.227817	521807.557288	40.696308
3520.335792	521537.726064	40.701312
3520.122793	521300.701793	40.706317
3519.740059	521042.669051	40.711322
3519.914714	520781.308411	40.716327
3519.440764	520537.741742	40.721332
3519.234255	520284.876750	40.726336
3519.367620	520036.706822	40.731341
3518.794891	519793.751424	40.736346
3518.774607	519537.862365	40.741351
3518.693652	519296.996055	40.746356
3518.239717	519050.016421	40.751360
3518.152839	518812.430584	40.756365
3517.538645	518588.324377	40.761370
3517.528893	518347.180099	40.766375
3517.252585	518111.788433	40.771380
3516.870516	517897.395469	40.776384
3517.324064	517661.275230	40.781389
3516.608087	517442.024067	40.786394
3516.630447	517226.597696	40.791399
3516.462989	517004.776169	40.796404
3516.027593	516791.439291	40.801408
3516.036820	516570.595450	40.806413
3515.466484	516371.838983	40.811418
3515.304645	516162.395391	40.816423
3514.981362	515961.167503	40.821428
3514.736482	515762.352325	40.826432
3515.058528	515568.502588	40.831437
3514.699103	515374.252566	40.836442
3514.468505	515191.460515	40.841447
3514.079999	514996.654376	40.846452
3513.947868	514817.838175	40.851456
3513.684548	514633.679645	40.856461
3513.428498	514471.417992	40.861466
3513.332994	514280.148215	40.866471
3513.061483	514120.111043	40.871476
3512.831365	513945.144999	40.876480
3512.657883	513785.948997	40.881485
3512.558112	513625.829399	40.886490
3512.631064	513466.035044	40.891495
3512.464754	513305.467696	40.896500
3511.944232	513155.323995	40.901504
3511.791430	512986.000888	40.906509
3511.278503	512854.416859	40.911514
3511.508197	512697.321898	40.916519
3511.318084	512565.229350	40.921524
3510.711018	512423.439044	40.926528
3511.149331	512289.171089	40.931533
3510.794767	512157.202519	40.936538
3510.975423	512020.292187	40.941543
3510.768911	511896.594092	40.946548
3510.719212	511764.726038	40.951552
3510.734192	511635.173691	40.956557
3510.343942	511518.988603	40.961562
3510.003482	511374.516903	40.966567
3510.126240	511250.964412	40.971572
3509.857589	511141.991480	40.976576
3510.014452	511015.497820	40.981581
3509.762175	510914.311360	40.986586
3509.713964	510801.709655	40.991591
3509.362399	510689.256332	40.996596
3509.391758	510578.107965	41.001600
3509.410183	510454.414426	41.006605
3509.194238	510355.141305	41.011610
3509.188102	510251.888423	41.016615
3509.167267	510142.111084	41.021620
3508.936675	510036.868766	41.026624
3508.993004	509935.172411	41.031629
3508.669462	509841.023000	41.036634
3508.783310	509729.703992	41.041639
3508.704495	509637.841996	41.046644
3508.497944	509549.338778	41.051648
3508.468296	509451.649920	41.056653
3508.111774	509360.639811	41.061658
3508.376147	509269.025153	41.066663
3508.451206	509174.707896	41.071668
3508.289529	509098.590595	41.076672
3508.166584	509002.077575	41.081677
3508.008563	508915.991920	41.086682
3507.744809	508823.345294	41.091687
3507.855275	508744.046565	41.096692
3507.821632	508652.728701	41.101696
3507.785089	508577.196451	41.106701
3507.427283	508496.047985	41.111706
3507.549128	508412.799506	41.116711
3507.768489	508344.764511	41.121716
3507.341528	508275.364125	41.126720
3507.440054	508188.525942	41.131725
3507.272551	508113.012358	41.136730
3507.184061	508042.140838	41.141735
3507.058719	507970.465303	41.146740
3507.119517	507907.563920	41.151744
3507.364797	507823.989509	41.156749
3506.838084	507755.108769	41.161754
3507.234893	507684.968636	41.166759
3507.116231	507621.841591	41.171764
3506.899065	507556.705966	41.176768
3506.859764	507489.467458	41.181773
3506.556161	507423.029439	41.186778
3506.685526	507355.915548	41.191783
3506.363587	507294.792783	41.196788
3506.673124	507232.203820	41.201792
3506.755112	507170.105990	41.206797
3506.379076	507108.991119	41.211802
3506.473436	507042.387540	41.216807
3506.472207	506990.877508	41.221812
3506.497133	506929.799829	41.226816
3506.773305	506876.626418	41.231821
3506.016389	506817.645319	41.236826
3506.247869	506757.192187	41.241831
3506.039452	506704.752647	41.246836
3506.133237	506664.965931	41.251840
3506.009724	506598.749290	41.256845
3506.200030	506553.532781	41.261850
3506.054798	506496.174337	41.266855
3506.297600	506437.236334	41.271860
3505.819977	506378.158995	41.276864
3505.909026	506339.536115	41.281869
3505.979451	506274.704429	41.286874
3505.682972	506230.070037	41.291879
3506.233405	506179.988461	41.296884
3506.213606	506130.351086	41.301888
3506.311921	506069.461194	41.306893
3505.769072	506025.674855	41.311898
3505.776835	505976.994133	41.316903
3505.654214	505921.451913	41.321908
3505.777560	505883.075614	41.326912
3505.978240	505830.366365	41.331917
3505.907931	505787.010766	41.336922
3505.693385	505734.366858	41.341927
3505.636493	505686.505196	41.346932
3505.566612	505645.982970	41.351936
3505.840680	505595.994004	41.356941
3505.524052	505550.247774	41.361946
3505.421578	505503.101267	41.366951
3505.629395	505456.664650	41.371956
3505.352846	505416.326369	41.376960
3505.385032	505368.297943	41.381965
3505.315188	505336.580145	41.386970
3505.415094	505280.241645	41.391975
3505.408024	505241.378504	41.396980
3505.631600	505200.808861	41.401984
3505.497430	505155.488200	41.406989
3505.065505	505118.311296	41.411994
3505.294317	505074.552414	41.416999
3505.583083	505031.087579	41.422004
3505.566752	505003.409143	41.427008
3505.482547	504944.720210	41.432013
3505.449124	504919.524015	41.437018
3505.372014	504865.590624	41.442023
3505.384044	504828.798385	41.447028
3505.312404	504795.055653	41.452032
3505.560270	504735.402623	41.457037
3505.589121	504710.145678	41.462042
3505.179208	504660.818820	41.467047
3505.548681	504621.641755	41.472052
3505.521041	504575.341231	41.477056
3505.394956	504545.300907	41.482061
3505.333597	504498.195801	41.487066
3505.275196	504451.039494	41.492071
3505.253381	504407.622204	41.497076
3505.114899	504382.441843	41.502080
3505.298111	504329.933266	41.507085
3504.936914	504307.419580	41.512090
3504.865373	504263.402504	41.517095
3504.987342	504228.059246	41.522100
3505.066649	504209.575026	41.527104
3505.225075	504164.559808	41.532109
3504.867060	504133.745713	41.537114
3505.154618	504104.448981	41.542119
3505.198046	504066.283764	41.547124
3504.952366	504035.502350	41.552128
3505.242458	503982.115501	41.557133
3505.367788	503953.704501	41.562138
3505.352698	503908.007535	41.567143
3504.937512	503870.471076	41.572148
3504.918675	503838.995549	41.577152
3505.169534	503785.563697	41.582157
3505.003350	503760.589258	41.587162
3504.859295	503728.981500	41.592167
3505.056824	503698.129441	41.597172
3504.853528	503667.998602	41.602176
3504.671159	503627.995582	41.607181
3504.775542	503593.666017	41.612186
3504.862390	503559.642813	41.617191
3504.973001	503537.711490	41.622196
3504.537392	503509.287216	41.627200
3504.705619	503469.987568	41.632205
3504.606268	503461.146662	41.637210
3504.990693	503417.662718	41.642215
3504.939590	503378.751803	41.647220
3504.644629	503350.811143	41.652224
3504.783547	503336.618447	41.657229
3504.801795	503296.734796	41.662234
3504.892344	503261.850058	41.667239
3504.804984	503231.042211	41.672244
3504.368801	503204.439513	41.677248
3504.888987	503167.259814	41.682253
3504.721102	503149.926989	41.687258
3504.729265	503107.918854	41.692263
3505.268344	503076.606836	41.697268
3504.718278	503044.404082	41.702272
3504.891045	503014.364518	41.707277
3504.585414	502975.695389	41.712282
3504.783003	502949.498244	41.717287
3504.897655	502916.380409	41.722292
3504.599687	502881.606941	41.727296
3505.137804	502847.004921	41.732301
3504.374236	502831.992847	41.737306
3504.920890	502800.274250	41.742311
3504.858719	502761.363724	41.747316
3504.657657	502740.189240	41.752320
3504.837441	502705.846030	41.757325
3504.678487	502684.158703	41.762330
3504.422339	502636.016551	41.767335
3504.684184	502618.463444	41.772340
3504.725394	502593.150897	41.777344
3504.714068	502555.041678	41.782349
3504.396471	502534.189041	41.787354
3504.539377	502495.599803	41.792359
3504.604472	502467.955122	41.797364
3504.522198	502459.819592	41.802368
3504.915018	502414.054282	41.807373
3504.638208	502392.790129	41.812378
3504.637095	502370.217049	41.817383
3504.842651	502331.313873	41.822388
3504.800627	502312.188875	41.827392
3504.706391	502271.865172	41.832397
3504.429914	502239.971999	41.837402
3504.708158	502222.567748	41.842407
3504.828207	502186.967640	41.847412
3504.256593	502163.370974	41.852416
3504.577911	502133.863185	41.857421
3504.489585	502109.582695	41.862426
3504.257002	502076.366332	41.867431
3504.613025	502054.394380	41.872436
3504.490237	502023.792486	41.877440
3504.515699	501997.975438	41.882445
3504.470559	501980.723293	41.887450
3504.545980	501951.355296	41.892455
3504.909929	501913.893980	41.897460
3504.309237	501903.663723	41.902464
3504.645565	501863.119193	41.907469
3504.700977	501831.476512	41.912474
3504.491822	501813.389682	41.917479
3504.660537	501777.781061	41.922484
3504.297225	501751.518959	41.927488
3504.351135	501727.215463	41.932493
3504.434710	501701.945563	41.937498
3504.018452	501691.989720	41.942503
3504.523899	501653.088272	41.947508
3504.498593	501639.325095	41.952512
3504.410668	501601.782700	41.957517
3504.426265	501584.267493	41.962522
3504.306893	501548.805180	41.967527
3504.321805	501527.898800	41.972532
3504.081598	501507.184567	41.977536
3504.411378	501480.356974	41.982541
3504.573712	501460.743217	41.987546
3504.494287	501444.811974	41.992551
3504.735110	501421.136519	41.997556
3504.485529	501400.069333	42.002560
3504.514316	501367.316489	42.007565
3504.667217	501341.427729	42.012570
3504.436390	501313.777408	42.017575
3504.370406	501290.453970	42.022580
3504.320354	501267.988456	42.027584
3504.855610	501226.955490	42.032589
3504.416550	501201.868720	42.037594
3504.509634	501178.013829	42.042599
3504.729947	501152.822769	42.047604
3504.380974	501133.947483	42.052608
3504.661495	501095.687768	42.057613
3504.533028	501069.893704	42.062618
3504.596011	501045.132293	42.067623
3504.471970	501008.201754	42.072628
3504.273703	500991.023468	42.077632
3504.659508	500963.477606	42.082637
3504.522017	500928.573707	42.087642
3504.418907	500909.608705	42.092647
3504.730282	500873.014001	42.097652
3504.656729	500850.399823	42.102656
3504.414458	500823.003636	42.107661
3504.595857	500802.981203	42.112666
3504.610692	500769.217116	42.117671
3504.637450	500742.385692	42.122676
3504.346517	500722.589679	42.127680
3504.665144	500693.991049	42.132685
3504.449440	500668.108956	42.137690
3504.216378	500645.114788	42.142695
3504.051443	500608.442974	42.147700
3504.208049	500612.062825	42.152704
3504.432244	500569.913303	42.157709
3504.406079	500555.238298	42.162714
3504.281581	500526.911914	42.167719
3504.080449	500504.266845	42.172724
3503.793486	500495.859060	42.177728
3504.015520	500471.223567	42.182733
3504.109473	500448.582404	42.187738
3504.137978	500430.810932	42.192743
3504.226584	500409.942212	42.197748
3504.383120	500387.088605	42.202752
3504.265991	500363.417708	42.207757
3504.371725	500345.077138	42.212762
3504.351948	500309.647235	42.217767
3504.461249	500293.178944	42.222772
3504.137969	500280.626050	42.227776
3504.432769	500250.157577	42.232781
3504.332683	500224.712137	42.237786
3503.891673	500203.218221	42.242791
3504.203824	500170.823344	42.247796
3504.083030	500164.413906	42.252800
3503.979469	500137.905888	42.257805
3504.027341	500123.066968	42.262810
3504.049397	500106.207341	42.267815
3504.140819	500083.920452	42.272820
3504.091613	500079.473827	42.277824
3504.095130	500051.784508	42.282829
3504.147204	500036.590516	42.287834
3504.132901	500016.598136	42.292839
3503.991805	499992.221860	42.297844
3504.128383	499979.039251	42.302848
3504.188801	499953.416196	42.307853
3503.943676	499927.183341	42.312858
3504.027529	499906.871605	42.317863
3504.228561	499889.376045	42.322868
3503.782065	499882.208066	42.327872
3504.077324	499857.053955	42.332877
3504.263509	499841.484258	42.337882
3504.051602	499824.408246	42.342887
3504.392258	499789.325303	42.347892
3504.285675	499778.155172	42.352896
3504.221304	499746.375865	42.357901
3504.347982	499730.157413	42.362906
3504.090234	499703.116297	42.367911
3504.366972	499679.129136	42.372916
3504.406222	499672.289260	42.377920
3504.116768	499630.319956	42.382925
3504.598447	499613.184733	42.387930
3504.307565	499583.820118	42.392935
3503.974052	499559.878634	42.397940
3503.839875	499546.536019	42.402944
3504.153045	499514.494143	42.407949
3504.386300	499504.181305	42.412954
3503.820720	499478.099685	42.417959
3503.971943	499460.763444	42.422964
3503.930264	499442.698357	42.427968
3504.063082	499425.719340	42.432973
3503.860232	499407.578451	42.437978
3503.857024	499378.370514	42.442983
3503.840945	499382.271017	42.447988
3503.475195	499372.052783	42.452992
3503.932669	499349.504637	42.457997
3503.817874	499344.764467	42.463002
3503.455717	499333.533212	42.468007
3503.988563	499299.937583	42.473012
3503.770977	499297.795353	42.478016
3503.906560	499278.841515	42.483021
3504.110248	499261.749898	42.488026
3503.755424	499237.507621	42.493031
3503.659310	499224.715591	42.498036
3503.825662	499218.311048	42.503040
3504.022541	499200.461121	42.508045
3503.825941	499186.773751	42.513050
3503.919627	499169.598190	42.518055
3504.265597	499135.323084	42.523060
3504.029531	499132.070067	42.528064
3504.098772	499108.266809	42.533069
3504.125473	499085.634555	42.538074
3503.960987	499072.650735	42.543079
3504.063353	499043.273699	42.548084
3504.290217	499044.857867	42.553088
3504.216557	499011.965036	42.558093
3504.000750	499002.380982	42.563098
3503.915546	498982.550525	42.568103
3503.848662	498955.528736	42.573108
3503.824060	498941.965861	42.578112
3504.125552	498918.125641	42.583117
3503.933505	498906.715362	42.588122
3503.941518	498888.034390	42.593127
3504.212750	498865.110094	42.598132
3503.959666	498854.418149	42.603136
3503.525971	498824.062405	42.608141
3503.948065	498826.324457	42.613146
3503.814222	498801.084824	42.618151
3504.280803	498770.434822	42.623156
3504.256477	498764.363996	42.628160
3504.186912	498743.619586	42.633165
3503.915549	498731.513007	42.638170
3504.086295	498701.365256	42.643175
3504.371597	498686.234504	42.648180
3503.830967	498679.941517	42.653184
3503.912030	498656.895145	42.658189
3504.065399	498637.887197	42.663194
3503.811999	498618.184170	42.668199
3504.399934	498600.474332	42.673204
3504.069172	498580.277255	42.678208
3503.969791	498562.625395	42.683213
3504.011789	498540.546899	42.688218
3504.073605	498527.678787	42.693223
3504.330167	498504.199488	42.698228
3504.330235	498495.340401	42.703232
3504.120435	498456.089456	42.708237
3504.335309	498430.591689	42.713242
3503.908123	498426.761263	42.718247
3504.139371	498395.439084	42.723252
3503.923848	498374.666694	42.728256
3503.816063	498358.990309	42.733261
3503.999409	498359.113312	42.738266
3503.836435	498332.763893	42.743271
3504.211126	498311.290648	42.748276
3503.672954	498293.049762	42.753280
3503.959607	498272.704125	42.758285
3504.072918	498259.017688	42.763290
3503.984749	498246.527454	42.768295
3504.238412	498220.162641	42.773300
3503.910742	498197.180286	42.778304
3504.123954	498177.048650	42.783309
3504.295870	498157.784141	42.788314
3504.053489	498143.850089	42.793319
3504.092998	498116.050851	42.798324
3503.895914	498094.870225	42.803329
3503.934689	498082.106687	42.808333
3503.916938	498058.163917	42.813338
3503.854776	498048.352568	42.818343
3504.221288	498033.259059	42.823348
3504.072960	498011.615002	42.828353
3503.897221	497995.746540	42.833357
3503.781951	497976.223479	42.838362
3503.636364	497963.083995	42.843367
3504.226854	497950.992540	42.848372
3503.926846	497930.081116	42.853377
3503.881259	497916.672664	42.858381
3504.313118	497894.329254	42.863386
3503.543584	497881.743963	42.868391
3503.784506	497855.380631	42.873396
3503.600188	497846.499744	42.878401
3504.011679	497825.273235	42.883405
3504.066519	497814.430750	42.888410
3503.772861	497799.087013	42.893415
3504.088687	497780.103110	42.898420
3503.886458	497769.250605	42.903425
3503.995383	497744.173625	42.908429
3504.208979	497732.951615	42.913434
3503.752738	497711.760876	42.918439
3503.840786	497686.990873	42.923444
3503.725783	497677.187675	42.928449
3503.696980	497657.650603	42.933453
3503.815062	497657.935806	42.938458
3503.789174	497639.360153	42.943463
3503.933496	497614.125519	42.948468
3503.714216	497619.931698	42.953473
3503.886333	497600.362806	42.958477
3503.907204	497572.008786	42.963482
3503.769161	497567.373075	42.968487
3503.759681	497536.593723	42.973492
3503.612223	497522.492308	42.978497
3503.715567	497512.198868	42.983501
3503.857132	497493.039703	42.988506
3503.522505	497487.878149	42.993511
3503.617562	497468.625056	42.998516
3503.663479	497473.832469	43.003521
3503.641669	497445.282490	43.008525
3503.748848	497436.456580	43.013530
3503.630554	497437.336045	43.018535
3503.924735	497417.292020	43.023540
3504.007060	497407.204351	43.028545
3503.934790	497384.231219	43.033549
3504.090808	497366.588447	43.038554
3503.948303	497344.031382	43.043559
3504.058423	497319.358643	43.048564
3503.839436	497309.217291	43.053569
3503.752513	497293.891074	43.058573
3504.017946	497271.522576	43.063578
3503.778483	497273.737513	43.068583
3503.809296	497257.531991	43.073588
3503.767343	497238.300309	43.078593
3503.600278	497221.315993	43.083597
3503.793990	497207.312288	43.088602
3503.672631	497196.699794	43.093607
3503.972617	497176.401447	43.098612
3503.592987	497157.476192	43.103617
3503.619414	497143.802646	43.108621
3503.918398	497121.226149	43.113626
3503.780004	497122.817595	43.118631
3503.690842	497093.163896	43.123636
3503.574980	497096.371874	43.128641
3503.492518	497081.247284	43.133645
3503.917257	497068.422025	43.138650
3503.734495	497046.427861	43.143655
3503.723236	497035.747241	43.148660
3503.544124	497036.383198	43.153665
3503.634636	497012.624445	43.158669
3503.547763	497005.449097	43.163674
3503.538509	497000.590371	43.168679
3503.741185	496982.180429	43.173684
3503.530795	496973.252605	43.178689
3503.512360	496963.636270	43.183693
3503.745546	496945.829007	43.188698
3503.662081	496938.551837	43.193703
3503.762527	496905.121367	43.198708
3503.563115	496909.304524	43.203713
3503.611229	496900.740832	43.208717
3503.837773	496876.859143	43.213722
3503.735529	496858.801043	43.218727
3503.620302	496853.452743	43.223732
3503.757840	496835.964263	43.228737
3503.833682	496826.839239	43.233741
3503.962073	496805.808173	43.238746
3503.805183	496801.884045	43.243751
3504.024092	496772.484900	43.248756
3504.064378	496774.200020	43.253761
3503.928709	496749.514727	43.258765
3504.109155	496737.892313	43.263770
3503.775373	496717.845516	43.268775
3504.254641	496696.758863	43.273780
3504.093650	496668.989097	43.278785
3504.038248	496649.252627	43.283789
3503.973823	496631.795873	43.288794
3503.515439	496613.540676	43.293799
3503.571115	496596.368680	43.298804
3503.861275	496599.816344	43.303809
3503.815756	496573.648315	43.308813
3503.625074	496563.653959	43.313818
3503.768543	496568.188031	43.318823
3503.957168	496529.933148	43.323828
3503.812251	496523.374337	43.328833
3503.882830	496507.668155	43.333837
3503.794321	496473.861723	43.338842
3503.292186	496481.079972	43.343847
3503.861185	496468.636526	43.348852
3503.798607	496442.369746	43.353857
3503.326848	496445.330314	43.358861
3503.633366	496425.890803	43.363866
3503.458089	496427.994436	43.368871
3503.622888	496382.806737	43.373876
3503.183293	496398.419685	43.378881
3503.026648	496376.724359	43.383885
3503.622319	496379.870626	43.388890
3503.311713	496381.033688	43.393895
3503.345868	496366.092589	43.398900
3503.110668	496354.890037	43.403905
3503.542765	496345.151532	43.408909
3503.909300	496336.030945	43.413914
3503.526563	496331.939893	43.418919
3503.542841	496306.116122	43.423924
3503.458884	496302.433508	43.428929
3503.556948	496298.874013	43.433933
3503.832447	496279.287358	43.438938
3503.431574	496273.882777	43.443943
3503.667609	496250.808849	43.448948
3503.586876	496254.264574	43.453953
3503.927162	496232.389270	43.458957
3503.918661	496223.226645	43.463962
3503.650628	496204.181494	43.468967
3503.928400	496191.277589	43.473972
3503.975896	496175.422878	43.478977
3503.817086	496166.182722	43.483981
3504.137114	496134.184411	43.488986
3503.975539	496116.793149	43.493991
3504.163378	496106.941234	43.498996
3503.978278	496079.630054	43.504001
3503.781456	496064.067018	43.509005
3503.757626	496036.679652	43.514010
3503.536226	496037.474219	43.519015
3504.038708	496017.598252	43.524020
3503.835162	496003.048843	43.529025
3503.719234	495986.105920	43.534029
3503.981760	495968.141172	43.539034
3503.745356	495952.432404	43.544039
3503.497073	495941.434189	43.549044
3503.715245	495942.260542	43.554049
3503.611757	495919.442386	43.559053
3503.953848	495899.895430	43.564058
3503.607552	495909.570199	43.569063
3503.879835	495883.148421	43.574068
3503.667099	495869.866139	43.579073
3503.452542	495871.368469	43.584077
3503.887305	495856.009212	43.589082
3503.396058	495835.024336	43.594087
3503.397189	495822.973999	43.599092
3503.852887	495813.231482	43.604097
3503.526702	495795.916564	43.609101
3504.016753	495778.421981	43.614106
3503.939145	495772.712996	43.619111
3504.154395	495746.958246	43.624116
3503.597116	495742.489596	43.629121
3503.650427	495731.747373	43.634125
3504.080880	495703.933281	43.639130
3503.856156	495687.614858	43.644135
3503.715616	495687.080232	43.649140
3503.778561	495655.729300	43.654145
3503.528900	495646.503240	43.659149
3503.777373	495641.603414	43.664154
3503.702264	495619.134820	43.669159
3503.891624	495598.750940	43.674164
3503.571912	495597.890208	43.679169
3503.570037	495577.739061	43.684173
3503.458045	495559.579949	43.689178
3503.468331	495564.034059	43.694183
3503.566103	495548.575915	43.699188
3503.593256	495546.141389	43.704193
3503.496378	495518.055941	43.709197
3503.671292	495505.319707	43.714202
3503.673850	495516.104084	43.719207
3503.802768	495483.831048	43.724212
3503.525280	495466.457488	43.729217
3503.590495	495465.839701	43.734221
3504.015442	495453.013278	43.739226
3503.791195	495429.960435	43.744231
3503.617465	495422.443764	43.749236
3503.516332	495420.738354	43.754241
3503.730679	495392.552887	43.759245
3504.007724	495376.002976	43.764250
3503.540203	495368.431454	43.769255
3504.050187	495345.414349	43.774260
3504.121451	495335.631078	43.779265
3503.417617	495321.919693	43.784269
3503.889933	495286.047735	43.789274
3503.646486	495292.719231	43.794279
3503.944215	495281.533048	43.799284
3503.624498	495252.520390	43.804289
3503.883714	495240.833939	43.809293
3503.977701	495238.388809	43.814298
3503.581334	495215.717333	43.819303
3503.962413	495202.593870	43.824308
3504.219775	495186.755763	43.829313
3503.608923	495166.953585	43.834317
3503.825867	495154.767430	43.839322
3503.729715	495134.124362	43.844327
3503.582880	495100.729672	43.849332
3503.767033	495097.409503	43.854337
3503.854346	495087.674196	43.859341
3503.678563	495054.790332	43.864346
3503.308418	495061.684472	43.869351
3503.750940	495057.665222	43.874356
3503.891804	495028.174339	43.879361
3503.527550	495025.194008	43.884365
3503.726482	495016.251158	43.889370
3503.306532	494996.722422	43.894375
3503.306628	494979.912127	43.899380
3503.438233	494974.574893	43.904385
3503.167462	494976.136814	43.909389
3503.316736	494967.758760	43.914394
3503.165879	494975.580313	43.919399
3503.139417	494967.685740	43.924404
3503.582648	494957.843473	43.929409
3503.632928	494935.556755	43.934413
3503.683541	494926.687939	43.939418
3503.450470	494933.459193	43.944423
3503.601000	494911.156600	43.949428
3503.713852	494887.087745	43.954433
3503.620255	494883.457002	43.959437
3503.914408	494872.625574	43.964442
3503.638834	494861.529753	43.969447
3503.793465	494842.821446	43.974452
3503.616026	494838.393800	43.979457
3503.233846	494821.441247	43.984461
3503.741246	494799.487183	43.989466
3503.265473	494799.359958	43.994471
3503.071869	494799.491938	43.999476
3503.357181	494796.358263	44.004481
3503.532278	494792.836934	44.009485
3503.468015	494762.162824	44.014490
3503.367285	494750.988665	44.019495
3503.229394	494756.884156	44.024500
3503.310791	494747.250872	44.029505
3503.402856	494744.552808	44.034509
3503.300739	494732.315535	44.039514
3503.304904	494717.884174	44.044519
3503.688287	494698.734487	44.049524
3503.684747	494700.406095	44.054529
3503.275607	494700.572144	44.059533
3503.222898	494674.858242	44.064538
3503.143579	494660.034954	44.069543
3503.129973	494660.189118	44.074548
3503.185540	494647.926865	44.079553
3503.385112	494659.845203	44.084557
3503.402199	494655.893112	44.089562
3503.564931	494658.449865	44.094567
3503.511828	494639.976725	44.099572
3503.686777	494620.859903	44.104577
3503.358346	494615.494010	44.109581
3503.948878	494603.957325	44.114586
3503.578141	494596.876532	44.119591
3503.259487	494574.799594	44.124596
3503.549310	494574.956434	44.129601
3503.422481	494565.355967	44.134605
3503.346228	494558.228612	44.139610
3503.320134	494543.447452	44.144615
3503.211536	494523.312013	44.149620
3503.645733	494531.902073	44.154625
3503.591460	494522.796466	44.159629
3503.604805	494513.123181	44.164634
3503.443183	494495.173398	44.169639
3503.415401	494481.050710	44.174644
3503.736294	494475.582142	44.179649
3503.379006	494489.259568	44.184653
3503.320307	494463.445046	44.189658
3503.607458	494458.791969	44.194663
3503.625674	494445.218970	44.199668
3503.439830	494446.564970	44.204673
3503.507904	494428.325639	44.209677
3503.560131	494404.670817	44.214682
3503.551261	494406.191389	44.219687
3503.163591	494407.366752	44.224692
3503.646712	494402.581414	44.229697
3503.320590	494374.732989	44.234701
3503.552403	494365.328906	44.239706
3503.206613	494366.649559	44.244711
3503.460180	494354.659626	44.249716
3503.553497	494360.822510	44.254721
3503.181944	494349.285831	44.259725
3503.475787	494332.276605	44.264730
3503.700275	494314.670700	44.269735
3503.508434	494311.814906	44.274740
3503.711392	494306.263657	44.279745
3503.231044	494287.756423	44.284749
3503.725745	494272.386370	44.289754
3503.207316	494279.304240	44.294759
3503.229024	494269.933319	44.299764
3503.393227	494258.868892	44.304769
3503.244111	494246.334910	44.309773
3503.273873	494227.291263	44.314778
3503.251752	494236.865034	44.319783
3503.399072	494227.018514	44.324788
3503.628770	494225.564515	44.329793
3503.531733	494218.288405	44.334797
3503.695011	494193.754950	44.339802
3503.431508	494196.328504	44.344807
3503.700279	494191.678265	44.349812
3503.892538	494169.114996	44.354817
3503.570400	494149.468624	44.359821
3503.793575	494139.863248	44.364826
3504.047712	494124.480461	44.369831
3503.627446	494104.798914	44.374836
3503.761666	494099.612922	44.379841
3503.685933	494080.940252	44.384845
3503.494605	494056.108210	44.389850
3503.514590	494053.775892	44.394855
3503.647524	494048.640725	44.399860
3503.524013	494036.862097	44.404865
3503.414998	494010.396620	44.409869
3503.734336	494007.915707	44.414874
3503.382221	494010.908384	44.419879
3503.368792	493997.188148	44.424884
3503.563998	493984.397016	44.429889
3503.704260	493967.209184	44.434893
3503.808722	493965.977506	44.439898
3503.419025	493947.759419	44.444903
3503.623403	493938.156909	44.449908
3503.870831	493926.927218	44.454913
3503.345386	493919.161702	44.459917
3503.949559	493904.989320	44.464922
3503.800444	493882.327749	44.469927
3503.475966	493875.087453	44.474932
3503.496939	493860.500851	44.479937
3503.436066	493854.434164	44.484941
3503.943074	493829.592709	44.489946
3503.351463	493837.281864	44.494951
3503.340375	493812.421003	44.499956
3503.486910	493799.333615	44.504961
3503.331996	493789.889093	44.509965
3503.521836	493790.922574	44.514970
3503.744793	493789.874702	44.519975
3503.442914	493776.554353	44.524980
3503.336035	493767.102227	44.529985
3503.116226	493762.326559	44.534989
3503.644885	493746.444331	44.539994
3503.644118	493751.508274	44.544999
3503.552972	493731.824943	44.550004
3503.593695	493716.424912	44.555009
3503.480007	493711.277995	44.560013
3503.590660	493704.779050	44.565018
3503.618542	493690.798869	44.570023
3503.817243	493664.486805	44.575028
3503.423008	493662.321185	44.580033
3503.497997	493658.916739	44.585037
3503.666738	493639.394781	44.590042
3503.375670	493621.717792	44.595047
3503.427778	493616.595281	44.600052
3503.614986	493621.933373	44.605057
3503.459513	493603.526009	44.610061
3503.576953	493579.150894	44.615066
3503.474708	493585.142399	44.620071
3503.394648	493571.128552	44.625076
3503.538834	493565.079995	44.630081
3503.384856	493550.419526	44.635085
3503.841849	493518.141820	44.640090
3503.955189	493529.720057	44.645095
3503.385463	493511.529993	44.650100
3503.744193	493488.281287	44.655105
3503.612736	493483.795408	44.660109
3503.639088	493480.044151	44.665114
3503.712001	493447.827031	44.670119
3503.729189	493443.722750	44.675124
3504.001059	493437.856521	44.680129
3503.781378	493412.319160	44.685133
3503.806822	493394.440011	44.690138
3503.853105	493397.825557	44.695143
3503.646718	493361.955853	44.700148
3504.064752	493352.319269	44.705153
3503.774268	493335.654677	44.710157
3503.685253	493312.425884	44.715162
3503.708655	493314.093360	44.720167
3503.719971	493302.748695	44.725172
3503.831923	493273.715316	44.730177
3503.574069	493267.730210	44.735181
3503.810837	493252.400080	44.740186
3503.667946	493237.079310	44.745191
3503.450536	493222.023498	44.750196
3503.581757	493214.103249	44.755201
3503.742743	493211.394068	44.760205
3503.921568	493190.198968	44.765210
3503.756303	493179.034054	44.770215
3503.618207	493164.674601	44.775220
3503.870490	493142.606977	44.780225
3503.473550	493135.681675	44.785229
3504.073402	493121.408100	44.790234
3503.952031	493102.589736	44.795239
3503.654146	493090.179759	44.800244
3503.841307	493078.503329	44.805249
3503.344078	493063.744812	44.810253
3503.564939	493047.201691	44.815258
3503.417250	493049.909014	44.820263
3503.652270	493043.238261	44.825268
3503.756702	493023.067510	44.830273
3503.661770	493013.866304	44.835277
3503.794346	492996.931980	44.840282
3503.783909	492978.045315	44.845287
3503.211846	492960.867861	44.850292
3503.762958	492951.463230	44.855297
3503.631125	492954.826372	44.860301
3503.650104	492927.123766	44.865306
3503.487019	492924.364488	44.870311
3503.779600	492909.582286	44.875316
3503.960270	492897.299095	44.880321
3503.423777	492885.078613	44.885325
3503.808051	492871.851712	44.890330
3503.508177	492870.683873	44.895335
3503.461249	492852.663719	44.900340
3503.649557	492825.643151	44.905345
3503.732908	492823.807059	44.910349
3503.589258	492801.092655	44.915354
3503.554302	492785.501251	44.920359
3503.634196	492775.613977	44.925364
3503.773913	492766.527478	44.930369
3503.398259	492767.852961	44.935373
3503.443245	492736.499892	44.940378
3503.555644	492732.734883	44.945383
3503.456584	492729.155217	44.950388
3503.619792	492726.243055	44.955393
3503.648419	492706.387780	44.960397
3503.764789	492688.696136	44.965402
3503.581219	492686.598380	44.970407
3503.770962	492671.325843	44.975412
3503.716007	492651.230520	44.980417
3503.401507	492639.633108	44.985421
3503.644973	492626.175087	44.990426
3503.940813	492610.885731	44.995431
3503.638224	492602.122265	45.000436
3503.771000	492589.947722	45.005441
3503.428741	492570.100284	45.010445
3503.638134	492545.304149	45.015450
3503.577452	492548.757399	45.020455
3503.517615	492546.184306	45.025460
3503.955787	492506.666232	45.030465
3503.426767	492518.245356	45.035469
3503.699206	492498.857725	45.040474
3503.626088	492489.197046	45.045479
3503.443260	492459.398735	45.050484
3503.821101	492448.957785	45.055489
3503.495120	492449.060062	45.060493
3503.848501	492435.179404	45.065498
3503.548456	492411.172584	45.070503
3503.680671	492405.226823	45.075508
3503.734824	492404.914529	45.080513
3503.433400	492387.744403	45.085517
3503.510288	492367.222805	45.090522
3503.405365	492363.036304	45.095527
3503.573050	492358.401585	45.100532
3503.762284	492339.786555	45.105537
3503.609233	492332.265349	45.110541
3503.425481	492328.547069	45.115546
3503.765009	492324.898000	45.120551
3503.573268	492293.733524	45.125556
3503.450985	492287.372182	45.130561
3503.174689	492273.894780	45.135565
3503.011262	492277.668167	45.140570
3503.218617	492285.383596	45.145575
3503.295637	492276.053562	45.150580
3503.294116	492250.935884	45.155585
3503.344077	492243.686401	45.160589
3503.310072	492232.348245	45.165594
3503.548579	492246.338282	45.170599
3503.665188	492239.989805	45.175604
3503.472437	492204.976604	45.180609
3503.126016	492203.461589	45.185613
3503.445345	492188.016248	45.190618
3503.530911	492181.875223	45.195623
3503.275221	492186.220268	45.200628
3503.473700	492176.060723	45.205633
3503.206210	492161.265170	45.210637
3503.437621	492149.935652	45.215642
3503.182016	492147.190882	45.220647
3503.242108	492151.486021	45.225652
3503.296237	492146.464066	45.230657
3503.109559	492152.874512	45.235661
3502.910607	492134.219350	45.240666
3503.185231	492129.871521	45.245671
3503.422530	492125.124458	45.250676
3503.208950	492106.167731	45.255681
3503.209704	492105.762589	45.260685
3503.287267	492098.458045	45.265690
3503.226795	492096.847181	45.270695
3503.021847	492103.412456	45.275700
3503.507920	492097.309381	45.280705
3503.143958	492083.136714	45.285709
3503.083631	492068.966684	45.290714
3503.376193	492057.374236	45.295719
3503.408334	492054.026910	45.300724
3503.850816	492051.323708	45.305729
3503.285877	492055.312530	45.310733
3503.476541	492025.353202	45.315738
3503.563243	492020.022214	45.320743
3503.316043	492015.301063	45.325748
3503.395737	492000.653072	45.330753
3503.342848	492010.334142	45.335757
3503.646832	491989.978800	45.340762
3503.659580	491966.023246	45.345767
3503.667592	491975.188289	45.350772
3503.754506	491954.664651	45.355777
3503.582485	491939.499336	45.360781
3503.391102	491918.867721	45.365786
3503.760367	491923.316612	45.370791
3503.565549	491908.205518	45.375796
3503.639749	491883.531153	45.380801
3503.585652	491879.539078	45.385805
3503.577535	491872.956980	45.390810
3503.410436	491856.980544	45.395815
3503.641832	491838.712844	45.400820
3503.487138	491825.772961	45.405825
3503.207698	491829.716703	45.410829
3503.546840	491824.750896	45.415834
3503.690251	491810.700393	45.420839
3503.342894	491806.805298	45.425844
3503.745114	491785.370714	45.430849
3503.406615	491805.073603	45.435853
3503.804218	491772.599680	45.440858
3503.774126	491749.005115	45.445863
3503.565180	491739.162944	45.450868
3503.731629	491731.337780	45.455873
3503.577705	491714.700785	45.460877
3503.671845	491692.403222	45.465882
3503.639000	491687.850676	45.470887
3503.154908	491675.975610	45.475892
3503.538613	491659.810656	45.480897
3503.629617	491653.972455	45.485901
3503.848188	491642.796588	45.490906
3503.467841	491641.742673	45.495911
3503.352435	491634.772306	45.500916
3503.812940	491612.669953	45.505921
3503.353756	491614.312575	45.510925
3503.463867	491600.722963	45.515930
3503.436841	491578.495058	45.520935
3503.368768	491572.580690	45.525940
3503.556962	491566.929672	45.530945
3503.677620	491571.215372	45.535949
3503.566847	491543.936355	45.540954
3503.386004	491533.279343	45.545959
3503.297552	491543.371423	45.550964
3503.430496	491523.346465	45.555969
3502.782687	491533.932110	45.560973
3503.197131	491529.410112	45.565978
3503.612513	491518.405634	45.570983
3503.279923	491496.884292	45.575988
3503.258684	491483.923076	45.580993
3503.128238	491488.349772	45.585997
3503.278296	491481.945107	45.591002
3503.300645	491487.107302	45.596007
3503.204819	491483.374954	45.601012
3503.255017	491464.375878	45.606017
3502.932283	491453.234814	45.611021
3503.222329	491445.136777	45.616026
3503.599064	491440.164927	45.621031
3503.340174	491447.144106	45.626036
3503.562973	491431.460180	45.631041
3503.559985	491431.663336	45.636045
3503.436654	491408.538868	45.641050
3503.192705	491404.272839	45.646055
3503.114624	491396.435542	45.651060
3503.753116	491388.788840	45.656065
3503.620096	491394.583341	45.661069
3503.260139	491370.230139	45.666074
3503.749454	491357.947790	45.671079
3503.582112	491347.085962	45.676084
3503.217063	491344.054509	45.681089
3503.358796	491320.837391	45.686093
3503.196134	491304.150766	45.691098
3503.268431	491307.988377	45.696103
3503.140501	491305.122012	45.701108
3503.618619	491300.944401	45.706113
3502.926133	491309.612769	45.711117
3503.162958	491295.141962	45.716122
3503.304887	491289.346241	45.721127
3503.258976	491288.138156	45.726132
3503.154968	491268.960680	45.731137
3503.225405	491262.011442	45.736141
3503.338422	491250.345584	45.741146
3503.457400	491260.658250	45.746151
3503.256741	491252.181897	45.751156
3503.684187	491238.086067	45.756161
3503.533629	491223.625792	45.761165
3503.248639	491210.351567	45.766170
3503.430001	491197.965857	45.771175
3503.317824	491207.302208	45.776180
3503.523730	491193.798447	45.781185
3503.523294	491177.795084	45.786189
3503.654667	491158.884154	45.791194
3503.381035	491158.775583	45.796199
3503.037211	491168.199212	45.801204
3503.704016	491148.342689	45.806209
3503.199686	491125.683246	45.811213
3502.938360	491123.698891	45.816218
3503.043541	491115.680576	45.821223
3503.386407	491114.562961	45.826228
3503.405906	491118.662178	45.831233
3503.029679	491121.811058	45.836237
3503.207680	491118.946952	45.841242
3503.576924	491102.226715	45.846247
3503.290380	491088.142339	45.851252
3503.487991	491072.968537	45.856257
3503.323087	491068.538003	45.861261
3503.282070	491074.469994	45.866266
3503.917705	491061.657879	45.871271
3503.499971	491042.580403	45.876276
3503.554269	491028.442108	45.881281
3503.390315	491033.330009	45.886285
3503.463018	491020.100399	45.891290
3503.536123	490997.400173	45.896295
3503.228924	491000.690096	45.901300
3503.222473	490984.940742	45.906305
3503.309738	490993.941807	45.911309
3503.168269	490984.696306	45.916314
3503.183538	490967.677388	45.921319
3503.321426	490986.039724	45.926324
3503.305823	490956.313860	45.931329
3503.466450	490945.602537	45.936333
3503.498599	490942.558879	45.941338
3503.700479	490929.460721	45.946343
3503.450176	490939.882579	45.951348
3503.619791	490903.847401	45.956353
3503.710944	490902.212467	45.961357
3503.546170	490911.506634	45.966362
3503.647538	490884.902149	45.971367
3503.465644	490872.674932	45.976372
3503.552223	490856.454960	45.981377
3503.389461	490870.610749	45.986381
3503.327164	490854.363663	45.991386
3503.285321	490823.578190	45.996391
3502.989585	490824.688592	46.001396
3503.365220	490802.396116	46.006401
3503.334895	490814.910370	46.011405
3503.580996	490816.441579	46.016410
3503.278312	490805.296957	46.021415
3503.272955	490792.636622	46.026420
3503.740760	490770.228248	46.031425
3503.544794	490772.994176	46.036429
3503.377161	490759.093337	46.041434
3503.619410	490764.879362	46.046439
3503.204026	490742.559911	46.051444
3503.594824	490723.556890	46.056449
3503.490962	490719.977595	46.061453
3503.380631	490730.630671	46.066458
3503.570563	490721.079431	46.071463
3503.352477	490691.233215	46.076468
3503.396507	490682.211471	46.081473
3503.179556	490685.132666	46.086477
3503.503810	490680.574075	46.091482
3503.739772	490676.586539	46.096487
3503.061229	490656.536982	46.101492
3503.439764	490633.332227	46.106497
3503.510615	490635.245671	46.111501
3503.407707	490628.323597	46.116506
3503.474206	490631.453225	46.121511
3503.434759	490609.378066	46.126516
3503.498998	490598.529843	46.131521
3503.453184	490580.406021	46.136525
3503.251636	490589.098411	46.141530
3503.610854	490576.177720	46.146535
3503.072890	490563.348187	46.151540
3503.468691	490544.040318	46.156545
3503.659464	490547.454192	46.161549
3503.559596	490542.253564	46.166554
3503.622063	490536.622109	46.171559
3503.097393	490512.192529	46.176564
3503.580248	490505.582989	46.181569
3503.786923	490490.913742	46.186573
3503.351458	490493.008523	46.191578
3503.472064	490468.578183	46.196583
3503.140317	490460.020898	46.201588
3503.134675	490452.222401	46.206593
3503.236461	490455.042604	46.211597
3503.098592	490446.353375	46.216602
3502.946276	490450.378604	46.221607
3503.161471	490437.987043	46.226612
3503.263974	490444.149780	46.231617
3503.153636	490449.434527	46.236621
3503.266719	490443.997628	46.241626
3503.065883	490419.972556	46.246631
3503.142675	490418.896957	46.251636
3503.295901	490404.843846	46.256641
3503.216870	490391.485837	46.261645
3503.117799	490407.860345	46.266650
3503.272669	490397.959959	46.271655
3503.337870	490412.232001	46.276660
3503.560927	490398.370432	46.281665
3503.318211	490376.732298	46.286669
3503.242713	490369.096746	46.291674
3503.435671	490353.062109	46.296679
3503.086102	490357.270476	46.301684
3503.123280	490353.567524	46.306689
3503.111018	490355.798012	46.311693
3503.287966	490352.630078	46.316698
3503.073743	490343.193174	46.321703
3503.048636	490333.878312	46.326708
3503.379577	490314.124642	46.331713
3503.253168	490312.118873	46.336717
3502.801772	490318.419849	46.341722
3503.386262	490302.728454	46.346727
3503.193253	490309.241824	46.351732
3503.152322	490305.551209	46.356737
3502.907354	490305.995212	46.361741
3503.080992	490306.575634	46.366746
3503.373700	490308.048872	46.371751
3502.935282	490297.533159	46.376756
3503.095261	490274.514445	46.381761
3503.156505	490276.429445	46.386765
3502.735488	490272.140496	46.391770
3503.386472	490264.542011	46.396775
3502.879757	490267.964891	46.401780
3503.217100	490267.303920	46.406785
3503.105720	490266.258056	46.411789
3503.223966	490257.426964	46.416794
3503.207452	490259.455549	46.421799
3503.242530	490269.376851	46.426804
3503.440231	490258.811215	46.431809
3503.485325	490239.001355	46.436813
3503.244051	490231.949064	46.441818
3503.445263	490217.331114	46.446823
3503.272973	490217.763631	46.451828
3503.302365	490218.265562	46.456833
3503.177423	490226.692778	46.461837
3503.011630	490211.271839	46.466842
3503.239759	490190.673294	46.471847
3503.076440	490194.599023	46.476852
3502.992136	490190.813948	46.481857
3503.250336	490180.339999	46.486861
3503.351032	490198.101226	46.491866
3503.297991	490183.016969	46.496871
3502.887816	490184.449378	46.501876
3502.990515	490177.342697	46.506881
3503.203648	490185.159378	46.511885
3503.161428	490190.382784	46.516890
3503.359623	490177.487271	46.521895
3502.987603	490167.619399	46.526900
3503.299873	490146.095862	46.531905
3503.606910	490136.930990	46.536909
3503.314032	490136.876100	46.541914
3503.587369	490130.046311	46.546919
3503.529186	490131.929556	46.551924
3503.337981	490111.346559	46.556929
3503.255104	490108.878064	46.561933
3503.142598	490102.261195	46.566938
3503.350146	490101.772675	46.571943
3503.299408	490094.588922	46.576948
3503.682372	490095.997264	46.581953
3503.435546	490074.258136	46.586957
3503.237975	490056.360382	46.591962
3503.582377	490056.711232	46.596967
3503.601979	490051.795467	46.601972
3503.550818	490035.444614	46.606977
3503.615684	490024.595960	46.611981
3503.587245	490010.520621	46.616986
3503.547726	490006.272604	46.621991
3503.183837	489985.666117	46.626996
3503.354339	489972.015129	46.632001
3503.659505	489963.154353	46.637005
3503.585142	489957.594999	46.642010
3503.843493	489950.058450	46.647015
3503.705751	489937.063929	46.652020
3503.386351	489930.682291	46.657025
3503.649095	489923.448922	46.662029
3503.614937	489897.472227	46.667034
3503.741507	489881.093147	46.672039
3503.327589	489879.335367	46.677044
3503.403963	489876.993613	46.682049
3503.576921	489865.317419	46.687053
3503.755870	489846.144406	46.692058
3503.511975	489834.837969	46.697063
3503.643737	489828.942109	46.702068
3503.717670	489808.468814	46.707073
3503.567128	489799.679992	46.712077
3503.575873	489785.902494	46.717082
3503.708714	489776.157206	46.722087
3503.350505	489760.867606	46.727092
3503.622476	489739.653862	46.732097
3503.634105	489746.185729	46.737101
3503.574805	489739.003192	46.742106
3503.830381	489704.978044	46.747111
3503.492251	489701.030398	46.752116
3503.642871	489687.129106	46.757121
3503.384176	489689.702514	46.762125
3503.070937	489673.038234	46.767130
3503.857496	489642.271824	46.772135
3503.628329	489654.210503	46.777140
3503.368167	489650.149225	46.782145
3503.591710	489629.854681	46.787149
3503.313416	489609.284898	46.792154
3503.538114	489608.439118	46.797159
3503.463098	489607.032930	46.802164
3503.553963	489590.963131	46.807169
3503.644109	489576.615481	46.812173
3503.457905	489567.123108	46.817178
3503.368016	489551.233791	46.822183
3503.250318	489559.761458	46.827188
3503.339851	489552.352731	46.832193
3503.540265	489522.489151	46.837197
3503.392404	489518.815283	46.842202
3503.170714	489508.670057	46.847207
3503.102429	489515.417230	46.852212
3503.458162	489502.395057	46.857217
3503.253388	489517.875372	46.862221
3503.189969	489514.086859	46.867226
3503.514195	489488.052950	46.872231
3503.359616	489489.495657	46.877236
3503.277886	489481.810081	46.882241
3503.347785	489482.001737	46.887245
3503.147436	489482.236110	46.892250
3503.143557	489472.714871	46.897255
3502.984029	489461.090980	46.902260
3503.272824	489439.063857	46.907265
3503.283855	489435.111614	46.912269
3503.140696	489436.653817	46.917274
3503.423599	489421.971688	46.922279
3503.355653	489442.444677	46.927284
3503.629270	489420.318634	46.932289
3503.648364	489409.527509	46.937293
3503.515244	489391.112444	46.942298
3503.419562	489388.747176	46.947303
3503.505803	489383.162266	46.952308
3503.310446	489368.555690	46.957313
3503.344488	489351.886881	46.962317
3503.333335	489333.452481	46.967322
3503.476798	489335.455879	46.972327
3503.215156	489335.851889	46.977332
3503.012262	489329.502280	46.982337
3503.232963	489337.875259	46.987341
3503.080136	489347.421557	46.992346
3503.372426	489315.669110	46.997351
3503.080246	489306.649199	47.002356
3503.558631	489291.936070	47.007361
3503.378890	489292.268485	47.012365
3503.194253	489296.856211	47.017370
3503.381484	489294.243616	47.022375
3503.061630	489276.212499	47.027380
3503.161842	489262.116264	47.032385
3503.480431	489254.114071	47.037389
3503.069573	489250.886916	47.042394
3503.067313	489245.873097	47.047399
3503.054063	489255.296080	47.052404
3502.905985	489253.850765	47.057409
3503.374052	489241.165201	47.062413
3503.292015	489252.928929	47.067418
3503.526715	489244.838694	47.072423
3503.265055	489222.797027	47.077428
3502.971649	489205.825300	47.082433
3503.055216	489204.292717	47.087437
3503.268987	489201.017471	47.092442
3503.243524	489183.699475	47.097447
3502.973147	489200.811205	47.102452
3502.950557	489188.000562	47.107457
3503.547858	489201.936171	47.112461
3502.973441	489194.986797	47.117466
3503.549299	489178.130893	47.122471
3503.254361	489170.124343	47.127476
3503.156377	489157.325596	47.132481
3503.329069	489161.552976	47.137485
3503.256295	489154.220397	47.142490
3503.355713	489140.377444	47.147495
3503.130966	489156.063813	47.152500
3503.371965	489144.123169	47.157505
3503.196951	489124.954721	47.162509
3503.298617	489110.554244	47.167514
3503.365191	489111.354227	47.172519
3503.474689	489109.766888	47.177524
3503.287265	489104.022553	47.182529
3503.242019	489114.463659	47.187533
3503.336820	489093.378491	47.192538
3503.522445	489071.367246	47.197543
3503.188877	489068.735640	47.202548
3503.285336	489062.541222	47.207553
3503.215701	489060.576995	47.212557
3503.246535	489068.068409	47.217562
3503.343521	489058.227117	47.222567
3503.322160	489039.439494	47.227572
3503.145281	489029.742776	47.232577
3503.266467	489022.784687	47.237581
3503.330169	489017.811031	47.242586
3503.462183	489009.635627	47.247591
3503.451938	489023.363500	47.252596
3503.130649	489002.445299	47.257601
3503.249997	488972.644312	47.262605
3503.054125	488974.954636	47.267610
3503.324237	488962.249524	47.272615
3503.293720	488970.307826	47.277620
3503.146864	488962.581681	47.282625
3503.262199	488965.754518	47.287629
3502.913127	488965.100703	47.292634
3503.040262	488978.553643	47.297639
3503.035256	488967.259573	47.302644
3502.976647	488970.105353	47.307649
3503.105516	488969.224042	47.312653
3503.072096	488963.961822	47.317658
3503.297478	488938.347980	47.322663
3503.237970	488932.431423	47.327668
3502.984813	488917.124530	47.332673
3503.130353	488927.687534	47.337677
3503.105252	488927.539660	47.342682
3503.372748	488921.014260	47.347687
3503.204449	488932.487922	47.352692
3503.160569	488931.684564	47.357697
3503.239885	488926.151264	47.362701
3502.831109	488920.087309	47.367706
3503.352627	488895.388954	47.372711
3503.080585	488896.039868	47.377716
3503.322654	488882.478080	47.382721
3503.267647	488880.815423	47.387725
3503.048442	488885.256761	47.392730
3503.337324	488877.968210	47.397735
3503.376748	488880.038753	47.402740
3503.395784	488868.386271	47.407745
3503.508469	488852.160442	47.412749
3503.146048	488848.317755	47.417754
3503.258338	488838.068726	47.422759
3503.259919	488839.892003	47.427764
3503.646484	488831.726937	47.432769
3503.572917	488822.115082	47.437773
3503.270954	488813.045830	47.442778
3503.484014	488787.433730	47.447783
3503.243892	488790.662782	47.452788
3503.539644	488797.960477	47.457793
3503.446647	488784.248979	47.462797
3503.389353	488775.292986	47.467802
3503.405516	488762.931784	47.472807
3503.229908	488773.140432	47.477812
3503.507073	488758.610646	47.482817
3503.512632	488754.405871	47.487821
3503.219937	488737.940116	47.492826
3503.331972	488715.737486	47.497831
3503.560998	488711.497379	47.502836
3503.231850	488706.281832	47.507841
3503.536644	488706.841575	47.512845
3503.432034	488696.170896	47.517850
3503.326317	488675.471512	47.522855
3503.415432	488671.861322	47.527860
3503.404049	488666.747489	47.532865
3503.537696	488670.018784	47.537869
3503.019475	488667.466958	47.542874
3503.642540	488627.810178	47.547879
3503.490720	488625.706942	47.552884
3503.243883	488622.656355	47.557889
3503.489614	488623.478691	47.562893
3503.190179	488626.717146	47.567898
3503.372507	488597.361470	47.572903
3502.983097	488587.900722	47.577908
3503.169317	488581.438703	47.582913
3503.119149	488574.659488	47.587917
3502.903669	488584.216074	47.592922
3503.544174	488572.870387	47.597927
3503.276929	488570.684087	47.602932
3503.291928	488588.561683	47.607937
3503.778541	488573.086928	47.612941
3503.431833	488546.701911	47.617946
3503.376312	488533.794727	47.622951
3503.106155	488544.879514	47.627956
3503.356683	488539.065781	47.632961
3503.326849	488529.953378	47.637965
3503.337752	488509.741891	47.642970
3503.198009	488492.188067	47.647975
3502.943271	488484.022916	47.652980
3503.256039	488493.698656	47.657985
3503.415496	488480.960061	47.662989
3503.315700	488489.890592	47.667994
3503.461925	488474.418908	47.672999
3503.245426	488460.524090	47.678004
3503.111088	488442.057638	47.683009
3503.519327	488441.233447	47.688013
3503.051696	488443.029624	47.693018
3503.558778	488444.317174	47.698023
3503.385171	488441.052376	47.703028
3502.965848	488450.337341	47.708033
3503.147416	488441.748646	47.713037
3503.042527	488420.744943	47.718042
3503.214840	488408.460131	47.723047
3503.177635	488406.085496	47.728052
3502.978986	488398.367306	47.733057
3503.471838	488383.245972	47.738061
3503.054360	488395.113907	47.743066
3503.331971	488390.663443	47.748071
3503.623966	488391.630432	47.753076
3503.094177	488384.775005	47.758081
3503.515130	488362.472479	47.763085
3503.584123	488352.331335	47.768090
3503.450123	488345.058770	47.773095
3503.386417	488351.197814	47.778100
3503.385949	488335.242686	47.783105
3503.573595	488314.597840	47.788109
3503.405645	488309.407354	47.793114
3503.427263	488295.424124	47.798119
3503.273361	488298.690283	47.803124
3503.546042	488298.545988	47.808129
3503.535470	488270.689201	47.813133
3503.447784	488266.651013	47.818138
3503.370567	488255.925103	47.823143
3503.378614	488257.443502	47.828148
3503.399471	488246.195564	47.833153
3503.850260	488213.808389	47.838157
3503.337497	488205.835858	47.843162
3503.178948	488191.779725	47.848167
3503.176238	488185.550043	47.853172
3503.261292	488182.396272	47.858177
3503.419467	488157.045255	47.863181
3503.126394	488148.430147	47.868186
3503.294340	488131.688443	47.873191
3503.263766	488136.353401	47.878196
3503.111477	488137.491934	47.883201
3503.387654	488125.089216	47.888205
3503.072980	488136.231930	47.893210
3503.029810	488133.402333	47.898215
3503.227102	488120.606862	47.903220
3502.865421	488108.051694	47.908225
3503.089627	488099.405453	47.913229
3503.468591	488104.968082	47.918234
3503.403591	488107.055215	47.923239
3503.371486	488118.153276	47.928244
3503.282478	488119.281807	47.933249
3503.583580	488113.409299	47.938253
3503.073319	488096.268239	47.943258
3502.820212	488087.849396	47.948263
3503.213622	488084.494911	47.953268
3502.990470	488081.947017	47.958273
3503.142321	488077.567010	47.963277
3502.532994	488083.336512	47.968282
3503.012736	488068.774177	47.973287
3503.030282	488090.704042	47.978292
3503.020991	488079.258161	47.983297
3503.139729	488073.161202	47.988301
3503.171895	488069.458595	47.993306
3503.208828	488072.137450	47.998311
3503.446666	488068.149070	48.003316
3503.148209	488074.021395	48.008321
3503.308591	488065.891751	48.013325
3503.106419	488051.487842	48.018330
3503.206947	488041.341546	48.023335
3503.536076	488035.717846	48.028340
3503.245768	488028.925740	48.033345
3503.380176	488029.461784	48.038349
3503.441025	488034.821453	48.043354
3503.445088	488011.368748	48.048359
3502.991118	488011.136699	48.053364
3503.168529	487993.025753	48.058369
3503.366078	487983.319965	48.063373
3503.208664	487998.236859	48.068378
3503.448837	487981.534258	48.073383
3503.434968	487991.261886	48.078388
3503.206377	487965.313261	48.083393
3503.346225	487939.255712	48.088397
3503.087948	487948.160895	48.093402
3503.283879	487931.414590	48.098407
3503.083584	487946.439608	48.103412
3503.169700	487940.094500	48.108417
3503.152846	487935.994391	48.113421
3502.949840	487942.155586	48.118426
3503.291701	487934.959606	48.123431
3503.353651	487923.147799	48.128436
3502.758281	487910.933356	48.133441
3503.238511	487888.671557	48.138445
3502.963442	487902.138186	48.143450
3503.334217	487889.416444	48.148455
3503.468696	487900.285689	48.153460
3503.075761	487893.003226	48.158465
3503.435083	487882.765287	48.163469
3502.823729	487898.564459	48.168474
3503.031657	487900.659127	48.173479
3503.225288	487892.777419	48.178484
3503.375071	487881.407581	48.183489
3503.220160	487857.726548	48.188493
3503.100334	487859.670416	48.193498
3503.292298	487841.658332	48.198503
3503.432222	487855.667235	48.203508
3503.168494	487854.797276	48.208513
3503.249923	487850.175083	48.213517
3503.358269	487842.104222	48.218522
3503.451026	487816.205906	48.223527
3503.592720	487809.497396	48.228532
3503.097488	487815.147637	48.233537
3503.372580	487798.692622	48.238541
3502.941927	487817.553146	48.243546
3503.190378	487801.912795	48.248551
3503.137617	487781.659941	48.253556
3503.039651	487768.201757	48.258561
3503.469283	487768.184611	48.263565
3503.389288	487769.261085	48.268570
3503.388965	487767.640339	48.273575
3503.555506	487756.824964	48.278580
3503.435705	487758.414264	48.283585
3503.321980	487731.180829	48.288589
3503.083229	487734.865723	48.293594
3503.082574	487727.419883	48.298599
3503.059950	487717.191574	48.303604
3503.129644	487727.817891	48.308609
3503.532341	487712.608967	48.313613
3503.068792	487727.523809	48.318618
3503.373637	487717.243737	48.323623
3503.404908	487695.913787	48.328628
3503.319104	487685.543486	48.333633
3503.304572	487681.088380	48.338637
3503.418837	487684.616177	48.343642
3503.602871	487671.974461	48.348647
3503.739615	487655.997072	48.353652
3503.377701	487642.529866	48.358657
3503.601357	487630.287088	48.363661
3503.159414	487637.144647	48.368666
3503.214548	487625.536348	48.373671
3503.132526	487621.142550	48.378676
3503.086760	487614.970140	48.383681
3503.217209	487588.913594	48.388685
3503.230851	487595.243272	48.393690
3503.301582	487581.201098	48.398695
3503.088929	487583.311628	48.403700
3502.918958	487579.286299	48.408705
3503.606687	487583.078047	48.413709
3503.345853	487574.660197	48.418714
3503.161107	487561.063621	48.423719
3503.469742	487537.764803	48.428724
3503.382140	487532.966635	48.433729
3503.263636	487531.009972	48.438733
3503.454463	487534.019156	48.443738
3503.541976	487525.242299	48.448743
3503.659365	487506.633837	48.453748
3503.505301	487498.756270	48.458753
3503.674648	487487.484412	48.463757
3503.344411	487498.477997	48.468762
3503.437996	487468.476097	48.473767
3503.407489	487449.941611	48.478772
3503.433921	487456.826510	48.483777
3503.452548	487446.743496	48.488781
3503.331511	487447.674513	48.493786
3503.534526	487432.851508	48.498791
3503.387417	487410.637656	48.503796
3503.257569	487407.517725	48.508801
3503.395195	487402.228035	48.513805
3503.163338	487399.580115	48.518810
3503.066914	487395.492467	48.523815
3503.141832	487397.253636	48.528820
3502.892693	487372.067262	48.533825
3503.309473	487356.399938	48.538829
3503.343147	487362.118674	48.543834
3503.237962	487353.270887	48.548839
3503.364288	487358.772361	48.553844
3503.388209	487356.489241	48.558849
3503.621142	487352.653451	48.563853
3503.219758	487337.925906	48.568858
3502.945332	487330.168602	48.573863
3503.352497	487315.465200	48.578868
3503.145135	487330.441168	48.583873
3503.327575	487312.936633	48.588877
3503.099886	487311.250478	48.593882
3503.080824	487315.559237	48.598887
3503.317238	487316.889650	48.603892
3502.958202	487318.364838	48.608897
3502.959627	487310.614579	48.613901
3502.940553	487281.086082	48.618906
3502.923505	487281.392814	48.623911
3503.117578	487273.156198	48.628916
3503.003152	487289.383873	48.633921
3502.961885	487273.231682	48.638925
3503.109021	487278.527272	48.643930
3502.941184	487264.623883	48.648935
3503.061235	487274.887911	48.653940
3502.829453	487273.708946	48.658945
3503.112677	487267.079184	48.663949
3503.237469	487264.780109	48.668954
3502.829108	487276.444681	48.673959
3503.045446	487262.632530	48.678964
3503.065645	487270.734193	48.683969
3503.146579	487270.974784	48.688973
3503.087797	487267.438359	48.693978
3503.108020	487276.451800	48.698983
3503.427285	487263.940401	48.703988
3503.235267	487264.528063	48.708993
3503.095111	487236.842204	48.713997
3503.223632	487229.527716	48.719002
3503.162370	487221.837984	48.724007
3503.279218	487221.768970	48.729012
3503.046581	487227.580495	48.734017
3503.258506	487217.922700	48.739021
3503.343148	487222.670980	48.744026
3503.335357	487220.342202	48.749031
3503.439219	487188.058770	48.754036
3503.117470	487178.282690	48.759041
3503.407603	487170.993289	48.764045
3502.921187	487173.096480	48.769050
3503.242433	487178.465887	48.774055
3503.335023	487173.385872	48.779060
3503.213607	487182.168471	48.784065
3503.039932	487167.303490	48.789069
3502.929889	487147.464253	48.794074
3503.242427	487141.032433	48.799079
3503.125615	487147.585500	48.804084
3503.188535	487135.570431	48.809089
3503.366881	487139.138856	48.814093
3503.490337	487136.333427	48.819098
3503.474250	487136.133460	48.824103
3503.517377	487132.276972	48.829108
3503.102204	487110.915621	48.834113
3503.481992	487098.141272	48.839117
3503.163453	487102.801346	48.844122
3503.385376	487098.562004	48.849127
3503.573519	487088.553316	48.854132
3503.324965	487081.146408	48.859137
3503.359591	487047.455337	48.864141
3503.352218	487043.860089	48.869146
3502.985165	487039.764486	48.874151
3503.327347	487039.355922	48.879156
3503.053684	487048.162648	48.884161
3503.646845	487035.455840	48.889165
3503.500018	487022.308782	48.894170
3503.216860	487021.137922	48.899175
3503.345089	486991.484381	48.904180
3502.897616	487002.294161	48.909185
3503.158910	486996.934156	48.914189
3503.205885	486998.953056	48.919194
3503.118650	486996.130253	48.924199
3503.074738	486992.844704	48.929204
3502.823694	487009.144869	48.934209
3503.264739	486998.792227	48.939213
3503.098656	486986.661295	48.944218
3502.846583	486967.502840	48.949223
3503.380363	486957.439450	48.954228
3502.790894	486965.080400	48.959233
3503.045617	486952.275066	48.964237
3502.747029	486955.817602	48.969242
3503.220532	486956.401389	48.974247
3503.240283	486955.689200	48.979252
3502.856510	486960.156998	48.984257
3503.398986	486951.155995	48.989261
3503.302994	486954.007986	48.994266
3502.989729	486954.158923	48.999271
3503.244758	486950.066282	49.004276
3503.073323	486952.372988	49.009281
3503.224513	486950.576257	49.014285
3503.110820	486930.889338	49.019290
3503.009082	486910.491329	49.024295
3503.173787	486911.630484	49.029300
3502.906680	486902.909392	49.034305
3503.440615	486904.952642	49.039309
3503.414370	486902.424119	49.044314
3503.079952	486905.516427	49.049319
3503.288742	486902.190918	49.054324
3503.408264	486899.335421	49.059329
3503.159236	486888.534584	49.064333
3503.381554	486878.317761	49.069338
3503.159848	486853.328985	49.074343
3503.405214	486862.610969	49.079348
3503.129924	486866.605740	49.084353
3503.360749	486850.460837	49.089357
3503.116898	486863.771298	49.094362
3503.005585	486847.123259	49.099367
3503.686318	486836.833955	49.104372
3503.179219	486816.803854	49.109377
3503.426354	486812.965711	49.114381
3503.409490	486811.094219	49.119386
3503.224054	486813.099219	49.124391
3503.581688	486800.986700	49.129396
3503.013234	486794.187458	49.134401
3503.378537	486779.946164	49.139405
3503.334073	486778.129688	49.144410
3503.265619	486770.896814	49.149415
3503.347937	486777.266565	49.154420
3503.226936	486774.347755	49.159425
3503.320790	486761.972969	49.164429
3503.073670	486744.485155	49.169434
3503.010003	486735.377237	49.174439
3503.173462	486721.319772	49.179444
3503.108109	486729.637812	49.184449
3503.186713	486727.396630	49.189453
3503.332171	486709.289513	49.194458
3503.202514	486729.927157	49.199463
3503.476557	486723.602594	49.204468
3503.306889	486715.321919	49.209473
3503.524331	486678.004713	49.214477
3503.452177	486689.667156	49.219482
3502.890704	486691.275701	49.224487
3503.580875	486681.238103	49.229492
3503.109771	486687.036830	49.234497
3503.507136	486672.942357	49.239501
3503.279395	486658.997337	49.244506
3502.974886	486637.972556	49.249511
3503.337922	486631.279302	49.254516
3503.115552	486637.038728	49.259521
3503.352964	486630.213361	49.264525
3503.337727	486634.420356	49.269530
3503.086266	486628.888015	49.274535
3503.107369	486631.822858	49.279540
3503.076082	486623.013706	49.284545
3503.039024	486609.342448	49.289549
3502.940217	486611.080494	49.294554
3502.771794	486603.762045	49.299559
3503.052499	486605.693386	49.304564
3503.044935	486600.173141	49.309569
3503.254777	486598.417764	49.314573
3502.965069	486600.844519	49.319578
3502.856900	486598.734156	49.324583
3503.221612	486596.143796	49.329588
3502.961232	486604.442062	49.334593
3503.154707	486606.285878	49.339597
3503.136461	486595.752334	49.344602
3503.152847	486610.896125	49.349607
3503.709854	486594.750104	49.354612
3503.135062	486582.683517	49.359617
3502.958197	486565.690998	49.364621
3503.385237	486563.901286	49.369626
3503.065144	486554.783158	49.374631
3503.414896	486549.864954	49.379636
3503.198158	486551.520333	49.384641
3503.149984	486552.794472	49.389645
3503.368907	486549.619271	49.394650
3502.985256	486544.411739	49.399655
3503.126095	486525.393359	49.404660
3503.070126	486507.469859	49.409665
3502.974588	486503.939103	49.414669
3503.203883	486508.462071	49.419674
3503.128650	486510.550996	49.424679
3503.338543	486505.553575	49.429684
3503.131319	486512.729031	49.434689
3503.336690	486514.267035	49.439693
3503.323820	486510.773870	49.444698
3503.268142	486498.422549	49.449703
3503.160867	486474.073725	49.454708
3503.139263	486464.199177	49.459713
3503.016500	486459.203668	49.464717
3503.192332	486459.935837	49.469722
3503.062092	486457.727634	49.474727
3503.328564	486454.646215	49.479732
3503.077011	486452.102589	49.484737
3503.258289	486454.708200	49.489741
3503.336684	486452.467018	49.494746
3503.159224	486440.489507	49.499751
3503.370227	486418.623146	49.504756
3503.034465	486422.171655	49.509761
3503.219009	486405.273838	49.514765
3503.491053	486403.559268	49.519770
3503.346682	486411.687309	49.524775
3503.276108	486400.706016	49.529780
3503.105874	486407.521066	49.534785
3502.927162	486395.543725	49.539789
3503.210705	486381.467028	49.544794
3503.066309	486370.649358	49.549799
3503.313751	486369.191959	49.554804
3502.861672	486370.529953	49.559809
3503.278631	486362.814941	49.564813
3503.589886	486364.336221	49.569818
3503.394880	486359.959990	49.574823
3503.447286	486359.445246	49.579828
3503.201077	486339.626690	49.584833
3503.101265	486329.916406	49.589837
3503.317039	486324.867351	49.594842
3503.077513	486325.614522	49.599847
3503.321173	486319.446600	49.604852
3503.065113	486325.312759	49.609857
3503.175595	486321.597432	49.614861
3503.194668	486325.393815	49.619866
3502.972988	486321.882963	49.624871
3503.270706	486313.224293	49.629876
3502.991249	486294.424089	49.634881
3503.081978	486283.619862	49.639885
3503.439910	486276.116775	49.644890
3503.590932	486274.573294	49.649895
3503.462047	486268.413585	49.654900
3503.312028	486277.505065	49.659905
3503.439825	486262.743698	49.664909
3503.440153	486242.734100	49.669914
3502.844575	486240.650082	49.674919
3503.497514	486227.224088	49.679924
3503.064457	486226.634102	49.684929
3503.120076	486231.691163	49.689933
3503.551824	486237.955204	49.694938
3503.199070	486223.269764	49.699943
3503.541640	486193.479789	49.704948
3503.043716	486193.406631	49.709953
3502.885484	486187.099561	49.714957
3503.130581	486178.753093	49.719962
3503.031670	486190.774674	49.724967
3503.532558	486167.899713	49.729972
3503.163695	486176.671229	49.734977
3503.376044	486172.382539	49.739981
3503.513629	486163.039907	49.744986
3503.242446	486155.433583	49.749991
3503.538636	486126.309383	49.754996
3503.211929	486131.325587	49.760001
3503.075050	486123.039472	49.765005
3503.526869	486115.977401	49.770010
3503.166014	486114.514818	49.775015
3503.664077	486095.287573	49.780020
3503.522570	486087.052831	49.785025
3503.684364	486078.364882	49.790029
3503.544431	486080.717370	49.795034
3503.320262	486057.247674	49.800039
3503.271495	486040.437071	49.805044
3503.201981	486050.630408	49.810049
3503.253418	486049.051993	49.815053
3503.611011	486050.920580	49.820058
3503.177644	486033.714841	49.825063
3503.184055	486013.349436	49.830068
3502.856483	486009.551316	49.835073
3502.894740	486003.263786	49.840077
3503.042775	485994.223368	49.845082
3502.891426	485991.410550	49.850087
3503.524249	485993.590245	49.855092
3503.106028	485994.568306	49.860097
3503.498449	485994.607704	49.865101
3503.157318	485992.686071	49.870106
3502.758222	486007.085486	49.875111
3503.209109	485988.777435	49.880116
3503.284843	485997.529415	49.885121
3503.132825	485975.162691	49.890125
3503.208588	485956.660613	49.895130
3503.040480	485954.559653	49.900135
3503.366891	485948.935771	49.905140
3502.985362	485946.209989	49.910145
3503.218894	485946.527793	49.915149
3503.557971	485938.166365	49.920154
3502.979445	485950.111933	49.925159
3503.213708	485940.146012	49.930164
3503.132166	485927.747752	49.935169
3503.338709	485905.678877	49.940173
3503.203106	485903.370141	49.945178
3503.414973	485909.618388	49.950183
3503.474986	485898.210899	49.955188
3503.368611	485899.392964	49.960193
3503.202318	485892.327196	49.965197
3503.401448	485876.743723	49.970202
3503.164385	485882.303064	49.975207
3503.210967	485864.666701	49.980212
3503.271233	485866.480987	49.985217
3503.221213	485866.438345	49.990221
3502.922059	485867.042983	49.995226
3503.165708	485864.370345	50.000231
3503.409023	485860.937883	50.005236
3503.299290	485843.478184	50.010241
3503.142239	485831.902332	50.015245
3503.653567	485812.824683	50.020250
3503.461591	485814.932137	50.025255
3503.359841	485822.395130	50.030260
3503.080110	485821.730237	50.035265
3503.102352	485799.842348	50.040269
3503.316076	485782.078172	50.045274
3502.967161	485779.296552	50.050279
3503.128584	485776.231630	50.055284
3503.037603	485781.615933	50.060289
3503.110319	485775.322881	50.065293
3503.178082	485767.358875	50.070298
3502.978453	485773.469576	50.075303
3503.243958	485764.258505	50.080308
3503.216259	485782.601416	50.085313
3503.349001	485767.940202	50.090317
3503.295495	485756.094644	50.095322
3502.932484	485740.498598	50.100327
3503.415380	485729.378776	50.105332
3503.130816	485721.166489	50.110337
3503.214292	485713.757223	50.115341
3503.615915	485719.468951	50.120346
3503.193591	485724.449716	50.125351
3503.121071	485714.836123	50.130356
3503.018709	485690.637500	50.135361
3503.133116	485690.467550	50.140365
3503.076401	485682.219231	50.145370
3502.903623	485682.449287	50.150375
3503.399069	485682.371084	50.155380
3503.279861	485686.544063	50.160385
3503.164186	485692.641519	50.165389
3503.158677	485671.669729	50.170394
3503.138481	485686.870693	50.175399
3503.378411	485688.251326	50.180404
3503.182990	485659.508077	50.185409
3502.983476	485650.573091	50.190413
3502.959895	485634.518034	50.195418
3502.930566	485637.612978	50.200423
3503.186033	485640.764223	50.205428
3503.459539	485636.516406	50.210433
3503.252470	485633.965638	50.215437
3503.349753	485629.998969	50.220442
3502.955643	485630.517305	50.225447
3503.377406	485635.769943	50.230452
3503.319142	485633.347631	50.235457
3503.364379	485600.665510	50.240461
3503.296410	485593.330796	50.245466
3503.217177	485610.972789	50.250471
3503.255228	485599.619253	50.255476
3503.107865	485593.614223	50.260481
3503.070813	485605.879689	50.265485
3503.324079	485597.177063	50.270490
3502.912587	485575.306817	50.275495
3503.390995	485548.837872	50.280500
3503.104802	485540.879060	50.285505
3503.035443	485542.612548	50.290509
3503.260281	485534.269002	50.295514
3502.749080	485547.673296	50.300519
3503.329056	485548.290960	50.305524
3503.295342	485548.853651	50.310529
3503.050736	485554.768893	50.315533
3503.211249	485533.466754	50.320538
3502.805766	485542.041711	50.325543
3503.064193	485537.542959	50.330548
3502.874634	485551.808275	50.335553
3503.144032	485542.393846	50.340557
3503.310668	485519.722925	50.345562
3503.164829	485506.979940	50.350567
3503.144846	485513.315624	50.355572
3503.044900	485505.074062	50.360577
3503.357246	485492.917216	50.365581
3503.765042	485500.350452	50.370586
3503.223502	485504.032974	50.375591
3503.445173	485482.771771	50.380596
3503.322955	485457.968080	50.385601
3503.235738	485451.953500	50.390605
3503.477426	485446.241545	50.395610
3503.231715	485456.361729	50.400615
3503.409527	485455.675160	50.405620
3503.349663	485427.518049	50.410625
3503.247030	485412.589812	50.415629
3503.425011	485407.850448	50.420634
3503.189947	485408.799586	50.425639
3503.399469	485410.691642	50.430644
3503.331890	485408.777369	50.435649
3503.462187	485388.645016	50.440653
3503.637337	485365.415311	50.445658
3503.505976	485366.803996	50.450663
3503.590740	485356.810744	50.455668
3503.429458	485353.543465	50.460673
3503.268012	485326.162157	50.465677
3503.461788	485326.283618	50.470682
3503.078877	485316.161628	50.475687
3503.316430	485308.170594	50.480692
3503.126774	485314.989101	50.485697
3503.422758	485314.334508	50.490701
3503.730665	485291.185048	50.495706
3503.349458	485279.745613	50.500711
3503.175267	485283.066152	50.505716
3503.273727	485264.661139	50.510721
3502.840082	485276.989502	50.515725
3503.260015	485263.498346	50.520730
3503.164974	485252.570922	50.525735
3503.452597	485215.543731	50.530740
3503.085667	485187.536125	50.535745
3502.852785	485133.923846	50.540749
3502.877499	485078.548245	50.545754
3502.587924	485020.030544	50.550759
3502.439027	484942.948578	50.555764
3502.512655	484864.716586	50.560769
3502.223909	484772.356406	50.565773
3502.344764	484671.926517	50.570778
3501.853330	484572.808769	50.575783
3502.411674	484455.590201	50.580788
3501.617297	484324.753897	50.585793
3501.504499	484183.169780	50.590797
3501.507782	484045.416678	50.595802
3500.530398	483892.567872	50.600807
3500.505973	483743.012374	50.605812
3500.537545	483571.255863	50.610817
3499.904414	483414.751687	50.615821
3499.880694	483233.121272	50.620826
3499.531484	483050.780617	50.625831
3499.273152	482854.135992	50.630836
3498.775363	482661.529904	50.635841
3498.436379	482460.536698	50.640845
3498.257267	482255.868059	50.645850
3497.908336	482034.199526	50.650855
3497.457266	481807.832398	50.655860
3497.174251	481596.079592	50.660865
3496.378513	481351.571271	50.665869
3496.162375	481123.284278	50.670874
3495.580217	480899.714247	50.675879
3495.777518	480643.588382	50.680884
3495.071560	480404.171919	50.685889
3494.220774	480151.347010	50.690893
3494.096287	479885.127464	50.695898
3493.457364	479632.110374	50.700903
3493.020352	479361.068387	50.705908
3492.832328	479092.415773	50.710913
3492.465273	478831.490668	50.715917
3491.674802	478531.607452	50.720922
3491.192603	478272.416221	50.725927
3490.904971	477970.569953	50.730932
3490.687339	477691.108435	50.735937
3489.632592	477398.750479	50.740941
3489.512045	477089.566480	50.745946
3488.961040	476786.274161	50.750951
3488.604461	476480.716475	50.755956
3488.220964	476177.033672	50.760961
3487.323424	475862.277004	50.765965
3486.985384	475541.294076	50.770970
3486.272845	475243.934135	50.775975
3485.490792	474915.560616	50.780980
3485.126414	474582.300427	50.785985
3484.234102	474271.370346	50.790989
3484.100882	473935.224430	50.795994
3483.546257	473620.074483	50.800999
3482.734575	473277.790088	50.806004
3482.132103	472966.185928	50.811009
3481.570968	472619.795562	50.816013
3481.058515	472282.212244	50.821018
3479.967026	471948.567638	50.826023
3479.575829	471617.392338	50.831028
3479.180507	471276.022529	50.836033
3478.153294	470941.185401	50.841037
3477.847823	470603.186905	50.846042
3476.621945	470266.342338	50.851047
3476.160491	469916.696702	50.856052
3475.429763	469593.248839	50.861057
3475.051875	469248.902217	50.866061
3474.317332	468909.422913	50.871066
3473.486004	468562.550846	50.876071
3473.104445	468219.353947	50.881076
3472.301684	467883.620777	50.886081
3471.643906	467554.704448	50.891085
3470.973239	467187.755824	50.896090
3470.653559	466857.101842	50.901095
3469.939134	466514.081804	50.906100
3469.287136	466170.742074	50.911105
3468.950021	465814.010551	50.916109
3468.276586	465463.309941	50.921114
3467.199731	465114.036495	50.926119
3466.802307	464760.136588	50.931124
3466.345578	464406.899437	50.936129
3465.616191	464057.503028	50.941133
3464.659690	463692.922629	50.946138
3464.001400	463348.422659	50.951143
3463.327068	462980.793376	50.956148
3462.465218	462637.937096	50.961153
3461.932715	462283.155453	50.966157
3461.679416	461940.546908	50.971162
3460.591079	461582.849272	50.976167
3459.824518	461227.225093	50.981172
3459.641344	460866.938011	50.986177
3458.427471	460528.060178	50.991181
3458.223581	460158.685527	50.996186
3457.316145	459817.922219	51.001191
3456.512214	459445.587000	51.006196
3455.810995	459099.808978	51.011201
3455.245051	458748.322873	51.016205
3454.571852	458394.261071	51.021210
3453.767209	458043.917446	51.026215
3453.179728	457683.337619	51.031220
3452.560630	457340.309071	51.036225
3451.980181	456988.695819	51.041229
3451.205454	456627.215301	51.046234
3450.495679	456277.386818	51.051239
3450.044911	455926.649463	51.056244
3449.211584	455571.756268	51.061249
3448.275857	455222.758734	51.066253
3447.756274	454864.354865	51.071258
3446.838665	454508.798646	51.076263
3446.203073	454159.838644	51.081268
3445.818429	453809.514422	51.086273
3444.576672	453472.664246	51.091277
3444.014409	453108.759621	51.096282
3443.383655	452762.618677	51.101287
3442.765678	452393.333074	51.106292
3441.698696	452043.444682	51.111297
3440.763041	451705.200702	51.116301
3440.373549	451359.101827	51.121306
3439.660316	451030.453741	51.126311
3439.158587	450677.968745	51.131316
3438.408559	450336.782880	51.136321
3437.539502	449994.443652	51.141325
3437.091339	449646.197033	51.146330
3436.393990	449311.229466	51.151335
3435.714966	448968.743553	51.156340
3434.908566	448633.326734	51.161345
3434.207881	448293.320976	51.166349
3433.649540	447950.141289	51.171354
3432.642218	447613.726605	51.176359
3431.866884	447276.813659	51.181364
3431.372442	446938.024409	51.186369
3430.557647	446604.000922	51.191373
3429.934392	446270.043930	51.196378
3429.099584	445949.920748	51.201383
3428.740666	445603.122557	51.206388
3428.169144	445276.807346	51.211393
3427.024277	444946.517817	51.216397
3426.444707	444605.221621	51.221402
3425.543380	444282.853218	51.226407
3424.816518	443955.427827	51.231412
3424.461735	443613.777403	51.236417
3423.710447	443285.433073	51.241421
3423.136081	442955.888805	51.246426
3422.514471	442634.063175	51.251431
3421.929790	442294.866928	51.256436
3421.111466	441974.535715	51.261441
3420.180952	441642.085642	51.266445
3419.618604	441304.801020	51.271450
3418.683401	440987.064227	51.276455
3417.928609	440659.040224	51.281460
3417.411041	440333.918730	51.286465
3416.566865	440012.347448	51.291469
3416.042078	439681.735677	51.296474
3415.646275	439361.201863	51.301479
3414.626907	439041.422462	51.306484
3414.115664	438710.541686	51.311489
3413.035255	438394.748949	51.316493
3412.686507	438067.438547	51.321498
3411.929387	437759.456031	51.326503
3411.170399	437426.490314	51.331508
3410.769662	437100.825511	51.336513
3409.828292	436787.503641	51.341517
3408.907245	436469.325751	51.346522
3408.093503	436149.806728	51.351527
3407.549102	435833.186009	51.356532
3406.937692	435525.787680	51.361537
3406.508520	435210.359541	51.366541
3405.715353	434886.886112	51.371546
3404.952014	434581.455242	51.376551
3404.045807	434262.358589	51.381556
3403.569574	433944.916429	51.386561
3402.784138	433640.747234	51.391565
3402.124225	433324.062697	51.396570
3401.329869	433015.723522	51.401575
3400.925922	432705.744694	51.406580
3400.297242	432384.117841	51.411585
3398.889787	432082.313703	51.416589
3398.600803	431760.650755	51.421594
3397.928695	431458.062875	51.426599
3397.171869	431147.283199	51.431604
3396.703198	430834.879911	51.436609
3395.721635	430533.345884	51.441613
3395.559660	430227.895217	51.446618
3394.514388	429912.270951	51.451623
3393.940425	429602.637437	51.456628
3393.141142	429294.280199	51.461633
3392.553332	428992.996290	51.466637
3391.978230	428685.739213	51.471642
3391.172608	428372.471041	51.476647
3390.481118	428063.930000	51.481652
3389.648395	427754.442671	51.486657
3388.860571	427460.385224	51.491661
3388.152697	427157.728044	51.496666
3387.035905	426853.227364	51.501671
3386.330896	426564.581743	51.506676
3386.023769	426264.797078	51.511681
3385.234997	425971.586882	51.516685
3384.909022	425682.033725	51.521690
3384.019372	425376.693043	51.526695
3383.408846	425082.733848	51.531700
3382.795802	424772.999553	51.536705
3381.792942	424487.502744	51.541709
3381.187258	424183.068834	51.546714
3380.264716	423896.638758	51.551719
3379.793013	423604.775125	51.556724
3379.233864	423305.708712	51.561729
3378.333331	423023.253731	51.566733
3377.781074	422728.929705	51.571738
3377.113850	422439.395982	51.576743
3376.148349	422147.315509	51.581748
3375.550397	421864.724578	51.586753
3374.761914	421569.307875	51.591757
3374.106231	421286.339144	51.596762
3373.607736	421007.940385	51.601767
3372.586976	420719.359020	51.606772
3371.956323	420433.253202	51.611777
3371.472844	420156.139068	51.616781
3370.805719	419865.257530	51.621786
3370.119078	419573.613967	51.626791
3369.329049	419290.087372	51.631796
3369.006668	419002.775053	51.636801
3368.107134	418722.105251	51.641805
3367.745274	418430.779551	51.646810
3366.591089	418145.978030	51.651815
3365.747339	417864.249320	51.656820
3365.231609	417574.742882	51.661825
3364.560385	417300.882208	51.666829
3364.176901	417016.430200	51.671834
3363.447430	416732.868456	51.676839
3362.605798	416452.395746	51.681844
3362.006000	416175.261059	51.686849
3360.975107	415897.150212	51.691853
3360.493121	415609.015916	51.696858
3360.036989	415336.067930	51.701863
3359.157195	415056.578531	51.706868
3358.717968	414776.356180	51.711873
3357.665654	414499.149941	51.716877
3357.464537	414215.886446	51.721882
3356.396842	413937.356089	51.726887
3355.516129	413659.936881	51.731892
3355.135198	413384.951453	51.736897
3354.536644	413105.373471	51.741901
3353.958779	412817.836544	51.746906
3352.966883	412549.647894	51.751911
3352.189555	412279.313890	51.756916
3351.787386	412000.507481	51.761921
3351.137109	411723.490970	51.766925
3350.623391	411448.127352	51.771930
3349.558318	411174.576284	51.776935
3349.241254	410894.500937	51.781940
3348.558080	410622.485287	51.786945
3347.247832	410350.744207	51.791949
3347.239054	410068.706554	51.796954
3346.465977	409788.210169	51.801959
3345.192707	409519.250998	51.806964
3345.003956	409241.325363	51.811969
3344.234956	408965.420268	51.816973
3343.241238	408702.025733	51.821978
3342.712949	408431.744705	51.826983
3342.054301	408162.447583	51.831988
3341.867945	407891.650259	51.836993
3340.598082	407630.882276	51.841997
3339.907186	407356.754613	51.847002
3339.511648	407081.891619	51.852007
3338.200466	406827.527628	51.857012
3337.780026	406553.756661	51.862017
3337.160668	406292.594898	51.867021
3336.419548	406023.825775	51.872026
3335.772173	405771.635440	51.877031
3335.125223	405500.483305	51.882036
3334.609588	405231.951239	51.887041
3334.001967	404980.841071	51.892045
3333.361595	404699.108057	51.897050
3332.471573	404445.572921	51.902055
3331.725146	404180.474073	51.907060
3331.061151	403913.072476	51.912065
3330.482816	403654.271302	51.917069
3329.684639	403398.730714	51.922074
3328.837584	403130.690604	51.927079
3328.074463	402877.656555	51.932084
3327.939710	402616.565452	51.937089
3326.635938	402368.874271	51.942093
3326.118673	402102.883009	51.947098
3325.678271	401845.544944	51.952103
3324.463098	401588.759451	51.957108
3324.005005	401340.545292	51.962113
3323.341888	401088.320073	51.967117
3322.905586	400832.371273	51.972122
3322.053943	400578.316303	51.977127
3321.295568	400322.592336	51.982132
3320.558349	400072.099417	51.987137
3319.719340	399835.576061	51.992141
3319.401926	399573.904521	51.997146
3318.698280	399316.791317	52.002151
3318.121699	399065.553496	52.007156
3317.385627	398815.254107	52.012161
3316.639667	398565.411946	52.017165
3316.116110	398319.777992	52.022170
3315.379728	398063.651561	52.027175
3314.775067	397812.027290	52.032180
3314.362482	397554.955967	52.037185
3313.476856	397307.007559	52.042189
3312.816400	397045.802349	52.047194
3312.167583	396787.186296	52.052199
3311.274564	396537.199564	52.057204
3310.810721	396276.948708	52.062209
3309.890288	396032.504624	52.067213
3309.467466	395773.921270	52.072218
3308.860378	395527.924016	52.077223
3307.931261	395282.764017	52.082228
3307.210140	395020.662824	52.087233
3306.153030	394781.188837	52.092237
3305.620461	394526.553941	52.097242
3305.505950	394283.520591	52.102247
3304.713799	394041.253707	52.107252
3304.296681	393787.332328	52.112257
3303.547174	393541.114395	52.117261
3302.749279	393284.198575	52.122266
3301.948129	393037.908926	52.127271
3301.372903	392780.979557	52.132276
3300.840557	392521.626100	52.137281
3299.876143	392277.619690	52.142285
3299.252095	392028.981129	52.147290
3298.794542	391780.772120	52.152295
3297.436138	391529.830690	52.157300
3297.183464	391276.958171	52.162305
3296.489652	391032.976516	52.167309
3295.504566	390789.395201	52.172314
3294.940623	390546.381253	52.177319
3293.730543	390323.453291	52.182324
3293.734986	390066.361394	52.187329
3292.911757	389831.520162	52.192333
3291.941752	389584.088634	52.197338
3291.590974	389354.814388	52.202343
3290.908830	389111.529575	52.207348
3290.427638	388865.719390	52.212353
3289.644049	388639.077206	52.217357
3289.149678	388392.401299	52.222362
3288.363636	388144.854405	52.227367
3287.066811	387910.711142	52.232372
3286.952355	387655.654962	52.237377
3286.167847	387436.761093	52.242381
3285.490104	387196.336064	52.247386
3284.844028	386950.259152	52.252391
3283.893710	386717.324815	52.257396
3283.757880	386475.715843	52.262401
3282.781103	386243.723556	52.267405
3282.302513	386006.666749	52.272410
3281.525157	385770.672864	52.277415
3280.885393	385537.809041	52.282420
3280.571362	385285.768605	52.287425
3279.734582	385050.771285	52.292429
3278.876266	384807.358322	52.297434
3278.260961	384565.253158	52.302439
3277.518930	384332.626794	52.307444
3276.590773	384086.422738	52.312449
3275.797631	383864.304606	52.317453
3275.224505	383618.321053	52.322458
3274.726124	383391.728412	52.327463
3273.869798	383169.361834	52.332468
3273.180715	382929.190553	52.337473
3272.628143	382700.720356	52.342477
3271.941445	382470.209977	52.347482
3271.229690	382235.989024	52.352487
3270.567614	382013.661213	52.357492
3269.796708	381771.181161	52.362497
3269.004498	381543.937238	52.367501
3268.485352	381312.223422	52.372506
3267.732967	381086.547328	52.377511
3267.044310	380866.633194	52.382516
3266.715319	380627.865564	52.387521
3265.773279	380397.154154	52.392525
3265.467978	380161.024986	52.397530
3264.983591	379936.673189	52.402535
3263.967420	379705.257227	52.407540
3263.287482	379477.856183	52.412545
3262.339732	379248.893804	52.417549
3262.083674	379008.273387	52.422554
3261.582332	378780.585685	52.427559
3260.690909	378551.559445	52.432564
3260.323265	378313.292419	52.437569
3259.454798	378084.234392	52.442573
3258.928802	377851.610792	52.447578
3257.975589	377616.458983	52.452583
3257.402435	377383.305947	52.457588
3256.865639	377152.536753	52.462593
3255.938696	376923.710191	52.467597
3255.111042	376682.123152	52.472602
3254.580041	376467.221172	52.477607
3253.725854	376240.592141	52.482612
3253.258927	375998.714998	52.487617
3252.801231	375776.955318	52.492621
3251.685942	375551.279428	52.497626
3250.988004	375317.803442	52.502631
3250.293242	375087.098248	52.507636
3250.013768	374867.492986	52.512641
3248.700972	374649.372732	52.517645
3248.284766	374424.139622	52.522650
3248.004976	374195.551369	52.527655
3246.841143	373972.774298	52.532660
3246.617945	373751.271752	52.537665
3245.887291	373527.635177	52.542669
3245.044353	373301.115201	52.547674
3244.471375	373070.964482	52.552679
3243.675267	372851.175790	52.557684
3243.084065	372630.335980	52.562689
3242.386218	372406.281153	52.567693
3241.648121	372180.705161	52.572698
3241.176787	371959.486700	52.577703
3240.232254	371745.515755	52.582708
3239.614625	371509.181790	52.587713
3238.994265	371290.883462	52.592717
3238.421797	371074.535273	52.597722
3237.701184	370849.661691	52.602727
3236.938420	370627.413884	52.607732
3236.323333	370404.938036	52.612737
3235.377860	370194.978913	52.617741
3235.038877	369960.169530	52.622746
3234.595465	369744.048572	52.627751
3233.598921	369525.622623	52.632756
3233.271177	369305.995826	52.637761
3232.158999	369081.581944	52.642765
3231.500196	368864.142289	52.647770
3231.073384	368642.467088	52.652775
3230.229126	368426.962651	52.657780
3229.842903	368196.832318	52.662785
3228.974748	367985.349192	52.667789
3228.068741	367760.514261	52.672794
3227.671394	367557.986317	52.677799
3226.770549	367333.555449	52.682804
3226.329527	367111.976511	52.687809
3225.666338	366896.817542	52.692813
3225.108811	366680.674013	52.697818
3224.728786	366456.970456	52.702823
3223.843877	366221.056985	52.707828
3223.260987	365992.218387	52.712833
3222.164777	365780.379159	52.717837
3221.477984	365568.194293	52.722842
3221.042911	365346.478422	52.727847
3220.080682	365126.117000	52.732852
3219.580437	364912.245741	52.737857
3218.806912	364698.289486	52.742861
3218.064862	364471.376582	52.747866
3217.745896	364261.264636	52.752871
3216.916125	364048.586395	52.757876
3216.232910	363825.350288	52.762881
3215.271232	363614.319294	52.767885
3214.706422	363397.932207	52.772890
3214.134901	363180.985396	52.777895
3213.314689	362972.804260	52.782900
3212.662295	362754.672366	52.787905
3211.752336	362540.447742	52.792909
3211.343964	362329.476015	52.797914
3210.825535	362122.388329	52.802919
3210.152902	361915.375010	52.807924
3209.553663	361704.481545	52.812929
3208.682789	361496.098268	52.817933
3207.861570	361274.983664	52.822938
3207.686780	361063.002374	52.827943
3206.632722	360853.805547	52.832948
3205.961022	360639.738120	52.837953
3205.370582	360434.486481	52.842957
3204.668835	360228.081066	52.847962
3204.038967	360016.930474	52.852967
3203.163476	359804.876310	52.857972
3202.923369	359589.616280	52.862977
3202.066328	359376.132330	52.867981
3201.178598	359171.914715	52.872986
3200.743362	358955.003273	52.877991
3199.809050	358756.364021	52.882996
3199.376908	358551.817256	52.888001
3198.829448	358338.941372	52.893005
3198.144414	358116.747361	52.898010
3197.377284	357911.640188	52.903015
3196.378106	357709.698847	52.908020
3195.841979	357500.507343	52.913025
3194.872494	357292.732212	52.918029
3194.414025	357088.972380	52.923034
3194.066890	356874.328053	52.928039
3193.069940	356676.631860	52.933044
3192.669332	356478.000767	52.938049
3192.012198	356270.400977	52.943053
3191.368746	356063.536148	52.948058
3190.849439	355852.884533	52.953063
3190.136427	355651.067702	52.958068
3189.511728	355432.847491	52.963073
3188.871318	355227.709226	52.968077
3187.731908	355025.651981	52.973082
3187.315509	354811.849605	52.978087
3186.446625	354603.869295	52.983092
3185.675982	354402.947323	52.988097
3185.343684	354207.528492	52.993101
3184.675957	353989.537953	52.998106
3184.341820	353783.658320	53.003111
3183.230556	353578.155307	53.008116
3182.650201	353368.546514	53.013121
3182.146273	353164.956262	53.018125
3181.257062	352965.116328	53.023130
3180.877868	352749.263573	53.028135
3179.942934	352541.718064	53.033140
3179.562724	352329.935675	53.038145
3178.751548	352128.018780	53.043149
3177.981396	351908.763260	53.048154
3177.594383	351702.883803	53.053159
3176.483222	351509.944951	53.058164
3175.907689	351298.138436	53.063169
3175.318297	351092.186835	53.068173
3174.592546	350897.835929	53.073178
3173.881017	350690.146031	53.078183
3173.224131	350485.500752	53.083188
3172.287993	350276.088705	53.088193
3171.812587	350090.577556	53.093197
3171.183483	349884.245857	53.098202
3170.878747	349675.546022	53.103207
3169.769134	349480.359971	53.108212
3169.318764	349267.660355	53.113217
3168.754293	349064.394919	53.118221
3167.950480	348866.587727	53.123226
3167.482155	348651.445242	53.128231
3166.411927	348457.216480	53.133236
3165.964423	348254.082263	53.138241
3165.263091	348058.164837	53.143245
3164.562105	347848.477258	53.148250
3163.825798	347645.615583	53.153255
3162.986010	347449.361602	53.158260
3162.474001	347244.910421	53.163265
3162.224422	347047.339959	53.168269
3161.314355	346854.098378	53.173274
3160.510776	346636.455968	53.178279
3160.184735	346441.160748	53.183284
3159.640780	346228.973423	53.188289
3158.781048	346030.172434	53.193293
3158.224738	345827.250318	53.198298
3157.590962	345611.715166	53.203303
3156.797058	345406.589315	53.208308
3156.023224	345200.721425	53.213313
3155.286855	344990.468952	53.218317
3154.558357	344789.123073	53.223322
3154.074810	344595.246445	53.228327
3153.239302	344398.930437	53.233332
3152.625059	344191.073829	53.238337
3151.964715	343987.449059	53.243341
3151.297612	343789.653525	53.248346
3150.751772	343590.489099	53.253351
3149.868236	343395.679119	53.258356
3149.192809	343181.490664	53.263361
3148.675491	342993.392144	53.268365
3147.766152	342792.271707	53.273370
3147.554788	342583.556659	53.278375
3146.453849	342390.712318	53.283380
3145.949893	342181.125824	53.288385
3145.158674	341994.772959	53.293389
3144.251402	341789.932525	53.298394
3144.150822	341591.938297	53.303399
3143.395964	341397.203321	53.308404
3142.717555	341200.215620	53.313409
3142.205828	340992.968105	53.318413
3141.351124	340796.847015	53.323418
3140.707573	340583.026182	53.328423
3139.825025	340390.624630	53.333428
3139.220461	340183.363642	53.338433
3138.605648	339992.267618	53.343437
3137.975053	339794.173317	53.348442
3137.336426	339585.541159	53.353447
3136.630438	339388.755732	53.358452
3136.054958	339191.083557	53.363457
3134.932683	338994.770063	53.368461
3134.447698	338796.904154	53.373466
3133.941517	338595.197171	53.378471
3133.047959	338403.784079	53.383476
3132.903092	338206.677114	53.388481
3131.933474	338005.601639	53.393485
3131.072156	337821.513029	53.398490
3130.474212	337616.915516	53.403495
3130.055669	337418.092983	53.408500
3129.495985	337223.670653	53.413505
3128.786365	337028.049567	53.418509
3128.086130	336823.262103	53.423514
3127.486414	336623.269375	53.428519
3126.563317	336433.789860	53.433524
3125.900388	336226.754467	53.438529
3125.323867	336033.273189	53.443533
3124.496640	335830.412006	53.448538
3124.152290	335632.768830	53.453543
3123.708344	335439.672169	53.458548
3122.727889	335234.949619	53.463553
3122.486948	335031.407744	53.468557
3121.530894	334834.520908	53.473562
3121.084316	334626.504440	53.478567
3120.118666	334423.355451	53.483572
3119.469274	334216.057175	53.488577
3118.882641	334015.240000	53.493581
3118.007108	333819.406719	53.498586
3117.182716	333626.212385	53.503591
3116.668148	333431.033703	53.508596
3115.977031	333233.998536	53.513601
3115.453738	333033.754029	53.518605
3114.700410	332833.214398	53.523610
3114.322635	332633.913125	53.528615
3113.435742	332447.777290	53.533620
3112.762506	332235.665335	53.538625
3112.370488	332038.401292	53.543629
3111.269178	331841.579899	53.548634
3110.691967	331649.893990	53.553639
3109.964580	331447.946140	53.558644
3109.060290	331255.419894	53.563649
3108.875079	331062.117427	53.568653
3108.489124	330867.675115	53.573658
3107.528686	330670.039022	53.578663
3106.647215	330471.982559	53.583668
3106.158238	330265.232914	53.588673
3105.918249	330071.045438	53.593677
3104.696430	329877.140112	53.598682
3104.202061	329679.834953	53.603687
3103.700493	329483.981579	53.608692
3102.831713	329279.987953	53.613697
3102.309365	329084.722383	53.618701
3101.434280	328887.144411	53.623706
3101.112793	328672.649685	53.628711
3100.207024	328481.211214	53.633716
3099.790736	328272.229595	53.638721
3098.702813	328077.381904	53.643725
3097.799227	327888.971291	53.648730
3097.873606	327686.504471	53.653735
3096.796714	327493.894010	53.658740
3096.044440	327293.211859	53.663745
3095.645811	327100.391251	53.668749
3094.841562	326907.201536	53.673754
3094.389404	326697.101103	53.678759
3093.190028	326510.999904	53.683764
3092.567666	326313.451737	53.688769
3092.143142	326109.430341	53.693773
3091.414492	325912.738184	53.698778
3091.067739	325725.227206	53.703783
3090.449976	325529.560435	53.708788
3089.427833	325327.261083	53.713793
3088.735011	325137.486601	53.718797
3087.796846	324939.781344	53.723802
3087.401090	324735.089941	53.728807
3086.251163	324559.313414	53.733812
3085.672995	324374.331085	53.738817
3085.065577	324175.018537	53.743821
3084.308289	323991.514962	53.748826
3083.792944	323797.762866	53.753831
3083.286694	323617.350433	53.758836
3082.616247	323429.681740	53.763841
3082.171081	323238.081430	53.768845
3081.134342	323047.287215	53.773850
3081.012402	322832.006887	53.778855
3080.000436	322649.100832	53.783860
3079.330035	322462.652131	53.788865
3079.128834	322273.506250	53.793869
3078.253093	322078.457804	53.798874
3077.700953	321876.177565	53.803879
3076.853850	321685.681310	53.808884
3076.177183	321495.514128	53.813889
3075.432664	321298.431700	53.818893
3074.863792	321103.867204	53.823898
3074.161584	320905.122188	53.828903
3073.356800	320717.392471	53.833908
3072.711344	320534.831368	53.838913
3072.357207	320334.018504	53.843917
3071.433965	320139.762601	53.848922
3070.755490	319954.277414	53.853927
3070.206085	319747.281406	53.858932
3069.528529	319557.263006	53.863937
3069.167714	319361.541474	53.868941
3068.069109	319168.813521	53.873946
3067.600318	318977.793316	53.878951
3066.834104	318790.970154	53.883956
3066.298806	318605.510504	53.888961
3065.793751	318403.240467	53.893965
3064.835817	318209.291526	53.898970
3064.263206	318012.913184	53.903975
3063.845828	317824.734298	53.908980
3063.064500	317623.015565	53.913985
3062.435482	317420.686658	53.918989
3061.567498	317231.737646	53.923994
3061.005037	317033.878842	53.928999
3060.142405	316837.467599	53.934004
3059.190465	316656.577025	53.939009
3058.778127	316459.533571	53.944013
3058.262614	316271.901913	53.949018
3057.640583	316080.467292	53.954023
3057.131518	315893.164914	53.959028
3056.427856	315698.686900	53.964033
3055.839448	315499.199472	53.969037
3054.791635	315305.997397	53.974042
3054.119066	315117.395355	53.979047
3053.761934	314931.314842	53.984052
3053.015419	314733.073169	53.989057
3052.292662	314535.413012	53.994061
3051.736022	314352.138540	53.999066
3051.037322	314152.716859	54.004071
3050.193780	313959.021570	54.009076
3049.749326	313766.561406	54.014081
3049.147282	313563.201897	54.019085
3048.158567	313379.535755	54.024090
3047.856667	313181.679109	54.029095
3047.038016	312991.288398	54.034100
3046.238745	312798.653459	54.039105
3045.613554	312600.133916	54.044109
3045.147183	312410.017454	54.049114
3044.301628	312215.657250	54.054119
3043.326764	312025.569668	54.059124
3042.924149	311831.546104	54.064129
3042.165363	311635.617830	54.069133
3041.589087	311457.587131	54.074138
3040.860910	311258.164750	54.079143
3040.085591	311067.763839	54.084148
3039.461097	310890.936694	54.089153
3039.281458	310705.839335	54.094157
3038.236226	310505.803734	54.099162
3037.787260	310317.106959	54.104167
3036.852654	310129.148814	54.109172
3036.349452	309921.769026	54.114177
3035.905719	309730.829586	54.119181
3034.680245	309547.983994	54.124186
3034.438193	309348.404965	54.129191
3033.308338	309173.896074	54.134196
3032.472739	308977.822636	54.139201
3032.233159	308783.335220	54.144205
3031.317450	308617.245937	54.149210
3030.700837	308426.662809	54.154215
3030.332532	308245.665820	54.159220
3029.467091	308053.237089	54.164225
3029.077592	307855.817984	54.169229
3028.176061	307689.088572	54.174234
3027.803153	307495.536952	54.179239
3027.108982	307295.160302	54.184244
3026.472583	307103.075826	54.189249
3025.785420	306916.677830	54.194253
3024.986930	306725.611581	54.199258
3024.226188	306532.832900	54.204263
3023.552136	306344.241984	54.209268
3022.682366	306157.820860	54.214273
3022.502564	305968.616399	54.219277
3021.457109	305791.211834	54.224282
3021.200844	305590.534034	54.229287
3020.495800	305405.435440	54.234292
3019.625382	305217.510628	54.239297
3018.693329	305034.102710	54.244301
3018.316666	304840.624129	54.249306
3018.018898	304653.677450	54.254311
3016.727994	304468.135525	54.259316
3016.104249	304269.576649	54.264321
3015.913261	304088.520343	54.269325
3014.985926	303903.684090	54.274330
3014.550518	303717.292716	54.279335
3013.982479	303522.594765	54.284340
3012.933888	303333.040316	54.289345
3012.388514	303144.984852	54.294349
3011.538748	302954.227003	54.299354
3011.123141	302770.632516	54.304359
3010.381863	302576.240834	54.309364
3009.787027	302393.183564	54.314369
3009.476770	302201.880954	54.319373
3008.255213	302025.492673	54.324378
3007.763533	301819.779020	54.329383
3007.048513	301634.167768	54.334388
3006.306864	301444.791509	54.339393
3005.883392	301251.086331	54.344397
3005.188989	301077.745858	54.349402
3004.280885	300882.181495	54.354407
3003.790502	300697.221151	54.359412
3003.022964	300510.547283	54.364417
3002.516090	300319.069727	54.369421
3001.444199	300138.504594	54.374426
3000.874699	299941.714025	54.379431
3000.775442	299762.904502	54.384436
2999.851952	299576.839969	54.389441
2999.404815	299383.110805	54.394445
2998.390399	299199.326760	54.399450
2997.992500	298996.548733	54.404455
2997.085816	298811.524817	54.409460
2996.704692	298624.303781	54.414465
2996.021602	298427.605810	54.419469
2995.213163	298249.416268	54.424474
2994.661167	298055.778594	54.429479
2994.174068	297864.651641	54.434484
2993.044581	297671.894426	54.439489
2992.866609	297481.915069	54.444493
2992.164598	297299.429307	54.449498
2991.723077	297094.720506	54.454503
2990.633886	296901.446756	54.459508
2989.838060	296709.246911	54.464513
2989.401881	296513.475504	54.469517
2988.584798	296333.961169	54.474522
2987.999593	296142.797019	54.479527
2987.268904	295951.502906	54.484532
2986.865069	295757.788432	54.489537
2986.321177	295568.323466	54.494541
2985.332859	295376.050888	54.499546
2984.580224	295175.183871	54.504551
2983.962919	295000.551838	54.509556
2983.102500	294813.657506	54.514561
2982.792234	294620.614732	54.519565
2982.232502	294436.906791	54.524570
2981.487367	294237.311027	54.529575
2981.012628	294038.894699	54.534580
2980.073620	293849.490687	54.539585
2979.761651	293654.002439	54.544589
2978.717681	293465.480594	54.549594
2978.079700	293275.595486	54.554599
2977.663108	293077.321879	54.559604
2976.792597	292884.366230	54.564609
2976.333866	292693.866505	54.569613
2975.722079	292502.754165	54.574618
2975.071308	292307.700385	54.579623
2974.046018	292113.622556	54.584628
2973.247843	291922.641116	54.589633
2972.961244	291736.009888	54.594637
2972.180301	291546.655342	54.599642
2971.611253	291351.944392	54.604647
2970.806719	291156.761213	54.609652
2969.855621	290969.419631	54.614657
2969.583557	290777.793734	54.619661
2968.657141	290595.286814	54.624666
2967.942474	290398.815449	54.629671
2967.495399	290210.247485	54.634676
2967.056913	290023.791845	54.639681
2966.199963	289833.098280	54.644685
2965.226280	289650.419919	54.649690
2964.837485	289446.026752	54.654695
2964.093772	289253.277443	54.659700
2963.436266	289077.985238	54.664705
2962.806165	288878.188589	54.669709
2962.137340	288692.965511	54.674714
2961.697117	288496.576695	54.679719
2960.914567	288305.997671	54.684724
2960.295708	288113.762672	54.689729
2959.966928	287918.018005	54.694733
2959.207496	287722.672470	54.699738
2958.970213	287524.391754	54.704743
2958.015437	287320.723431	54.709748
2956.972928	287130.286719	54.714753
2956.546528	286932.519473	54.719757
2955.680559	286734.821697	54.724762
2955.161014	286538.953596	54.729767
2954.697033	286347.737229	54.734772
2953.825273	286152.535902	54.739777
2953.109625	285958.328476	54.744781
2952.345929	285761.327073	54.749786
2951.575765	285562.161807	54.754791
2951.245277	285379.761210	54.759796
2950.448050	285191.373019	54.764801
2949.257075	284985.957996	54.769805
2948.831320	284805.533258	54.774810
2948.421771	284605.597315	54.779815
2947.680590	284416.741467	54.784820
2947.018789	284222.906686	54.789825
2946.731610	284019.640242	54.794829
2945.504568	283837.431835	54.799834
2944.867218	283633.660353	54.804839
2944.467501	283447.831683	54.809844
2943.531605	283261.731268	54.814849
2943.216270	283071.534036	54.819853
2942.459312	282877.026117	54.824858
2942.042600	282675.384099	54.829863
2941.098044	282484.165660	54.834868
2940.617204	282299.062518	54.839873
2940.205056	282090.517670	54.844877
2938.970292	281897.434853	54.849882
2938.145410	281704.465361	54.854887
2938.070543	281507.760577	54.859892
2936.985021	281324.815780	54.864897
2936.808995	281123.899159	54.869901
2936.002850	280929.653046	54.874906
2935.330705	280739.002159	54.879911
2934.647799	280541.985852	54.884916
2933.614779	280350.093109	54.889921
2933.152185	280155.665053	54.894925
2932.409731	279963.853553	54.899930
2931.727572	279762.583717	54.904935
2931.339311	279568.296559	54.909940
2930.553860	279386.220632	54.914945
2930.114900	279181.830490	54.919949
2929.247412	278995.565198	54.924954
2928.801848	278799.300421	54.929959
2927.984816	278598.331834	54.934964
2927.216317	278406.982564	54.939969
2926.934257	278220.624453	54.944973
2926.186526	278019.237300	54.949978
2925.473377	277815.221399	54.954983
2924.645497	277620.646928	54.959988
2923.749303	277421.880966	54.964993
2923.368561	277231.998240	54.969997
2922.860066	277039.792628	54.975002
2921.898116	276833.600242	54.980007
2921.119417	276635.095743	54.985012
2920.357205	276445.629893	54.990017
2920.082031	276238.793887	54.995021
2919.030849	276049.424695	55.000026
2918.403528	275856.524687	55.005031
2918.073532	275665.997093	55.010036
2917.194831	275474.817781	55.015041
2916.643440	275283.408364	55.020045
2915.955108	275089.753937	55.025050
2915.379365	274895.572314	55.030055
2914.763617	274703.434496	55.035060
2913.646396	274505.238192	55.040065
2913.807599	274299.835680	55.045069
2912.941838	274113.034880	55.050074
2911.605933	273919.330183	55.055079
2911.681678	273735.079983	55.060084
2910.789989	273534.683194	55.065089
2910.171605	273335.873123	55.070093
2909.150233	273136.744844	55.075098
2908.444767	272941.412292	55.080103
2908.151579	272749.962082	55.085108
2907.620803	272565.807993	55.090113
2907.039440	272352.500647	55.095117
2906.364067	272161.976934	55.100122
2905.480484	271968.888437	55.105127
2904.914455	271768.261991	55.110132
2904.044307	271567.429041	55.115137
2903.509646	271364.632881	55.120141
2902.732652	271173.819780	55.125146
2902.189598	270980.601116	55.130151
2901.471238	270790.390039	55.135156
2900.759137	270595.109808	55.140161
2900.319158	270389.319049	55.145165
2899.906161	270198.066477	55.150170
2898.848879	269997.441741	55.155175
2898.177063	269800.347054	55.160180
2897.458924	269606.061264	55.165185
2897.145401	269405.802813	55.170189
2896.103230	269218.215651	55.175194
2895.860883	269025.994015	55.180199
2895.433610	268813.579897	55.185204
2894.148010	268623.306331	55.190209
2893.650687	268409.986575	55.195213
2893.419316	268213.739449	55.200218
2892.472805	268020.432590	55.205223
2891.751204	267818.227236	55.210228
2891.070518	267617.008735	55.215233
2890.164721	267413.049913	55.220237
2889.223018	267234.539594	55.225242
2888.847545	267040.658760	55.230247
2888.384611	266841.392589	55.235252
2887.348668	266656.453936	55.240257
2886.859636	266443.846727	55.245261
2886.233815	266255.888980	55.250266
2885.339639	266066.496646	55.255271
2885.038249	265876.883188	55.260276
2884.281440	265680.873014	55.265281
2883.811585	265478.272184	55.270285
2882.705160	265281.808181	55.275290
2882.477873	265095.163095	55.280295
2881.759636	264882.923999	55.285300
2881.024989	264694.296512	55.290305
2880.668962	264498.707320	55.295309
2879.913612	264300.532776	55.300314
2878.984691	264095.229299	55.305319
2878.539272	263894.051599	55.310324
2877.684794	263706.309480	55.315329
2877.352077	263507.533606	55.320333
2876.378779	263312.832274	55.325338
2875.611717	263112.928398	55.330343
2875.371666	262907.873069	55.335348
2874.362214	262715.087893	55.340353
2874.206684	262516.717483	55.345357
2873.503293	262325.514017	55.350362
2872.598099	262117.712085	55.355367
2871.991462	261911.518426	55.360372
2871.372756	261721.728112	55.365377
2870.671698	261504.980511	55.370381
2869.616949	261315.412297	55.375386
2869.030805	261121.007523	55.380391
2868.633643	260912.260054	55.385396
2867.681662	260726.929064	55.390401
2867.168339	260532.385810	55.395405
2866.450796	260329.954560	55.400410
2865.794061	260139.279912	55.405415
2865.138513	259939.258561	55.410420
2864.378571	259735.612007	55.415425
2864.077501	259536.808207	55.420429
2863.212423	259340.742496	55.425434
2862.565656	259140.032723	55.430439
2861.863906	258937.014260	55.435444
2861.000197	258744.565182	55.440449
2860.443362	258544.860337	55.445453
2859.909623	258351.085932	55.450458
2859.200277	258157.084810	55.455463
2858.932958	257959.422930	55.460468
2857.970535	257762.966381	55.465473
2857.591102	257558.904777	55.470477
2856.828239	257352.841202	55.475482
2855.902654	257160.403176	55.480487
2855.427420	256956.713811	55.485492
2854.579846	256753.745740	55.490497
2854.270944	256557.415933	55.495501
2853.510928	256355.885995	55.500506
2852.671334	256154.699917	55.505511
2852.101710	255946.111230	55.510516
2851.104962	255757.684046	55.515521
2850.866424	255552.965270	55.520525
2850.169138	255356.519777	55.525530
2849.442661	255150.172355	55.530535
2849.004736	254946.657235	55.535540
2848.434675	254752.611548	55.540545
2847.406710	254551.100291	55.545549
2846.875182	254352.821345	55.550554
2846.111060	254145.003814	55.555559
2845.647827	253942.716135	55.560564
2844.649137	253750.394654	55.565569
2844.322284	253538.510205	55.570573
2843.474729	253337.531899	55.575578
2842.451152	253142.031601	55.580583
2842.053578	252927.153935	55.585588
2841.407980	252738.088264	55.590593
2840.879921	252537.747828	55.595597
2840.115206	252343.480722	55.600602
2839.404509	252135.988007	55.605607
2838.954562	251932.503454	55.610612
2838.069527	251741.795931	55.615617
2837.639252	251533.062575	55.620621
2836.860044	251337.500058	55.625626
2836.111037	251137.730983	55.630631
2835.434374	250927.178307	55.635636
2834.567914	250734.176953	55.640641
2834.363094	250544.534496	55.645645
2833.280320	250344.437208	55.650650
2832.551948	250141.762856	55.655655
2832.129775	249937.155745	55.660660
2831.512669	249754.735554	55.665665
2830.891164	249541.221787	55.670669
2830.325363	249345.907933	55.675674
2829.197285	249153.459190	55.680679
2828.609122	248942.945968	55.685684
2828.289827	248749.911243	55.690689
2827.376792	248554.551488	55.695693
2826.841085	248359.616084	55.700698
2826.074768	248163.520534	55.705703
2825.592438	247962.618095	55.710708
2824.957673	247766.731418	55.715713
2824.408993	247559.371629	55.720717
2823.687443	247367.853915	55.725722
2822.837737	247159.676507	55.730727
2822.283519	246954.432118	55.735732
2821.395337	246761.770144	55.740737
2821.026591	246569.433620	55.745741
2820.582211	246367.712424	55.750746
2819.583601	246160.502265	55.755751
2819.328262	245956.205129	55.760756
2818.311718	245764.226934	55.765761
2817.609287	245550.095010	55.770765
2816.917534	245355.035521	55.775770
2816.185243	245155.322513	55.780775
2816.142488	244953.055897	55.785780
2814.917208	244760.832029	55.790785
2814.486511	244550.376601	55.795789
2813.726001	244346.874882	55.800794
2813.025496	244145.604930	55.805799
2812.673801	243935.036096	55.810804
2811.926629	243744.698808	55.815809
2811.218288	243535.180243	55.820813
2810.813203	243332.515085	55.825818
2809.590406	243133.468484	55.830823
2809.371320	242926.521808	55.835828
2808.417335	242730.514553	55.840833
2807.816812	242519.401724	55.845837
2807.073267	242317.326542	55.850842
2806.423694	242120.762722	55.855847
2806.217668	241910.403322	55.860852
2805.053575	241710.585717	55.865857
2804.355154	241506.874947	55.870861
2803.955586	241305.332632	55.875866
2803.145039	241097.209413	55.880871
2802.626068	240897.876661	55.885876
2801.788588	240699.740596	55.890881
2801.154449	240489.909815	55.895885
2800.409564	240290.562924	55.900890
2799.579621	240095.507898	55.905895
2799.446755	239881.931901	55.910900
2798.541930	239690.225270	55.915905
2797.965483	239481.736772	55.920909
2797.042633	239273.940123	55.925914
2796.461001	239079.611411	55.930919
2795.951199	238884.685974	55.935924
2795.241441	238686.915070	55.940929
2794.652666	238480.773069	55.945933
2794.019971	238276.369970	55.950938
2793.412435	238080.417369	55.955943
2792.677187	237870.327279	55.960948
2792.118714	237661.711974	55.965953
2791.271658	237463.735810	55.970957
2790.542548	237258.840582	55.975962
2789.825972	237051.320969	55.980967
2789.281193	236854.698559	55.985972
2788.725159	236653.112839	55.990977
2788.010359	236447.325652	55.995981
2787.207365	236241.782006	56.000986
2786.619235	236041.653962	56.005991
2786.146437	235842.959461	56.010996
2785.492388	235645.821859	56.016001
2784.645595	235428.649873	56.021005
2784.121172	235223.878939	56.026010
2783.218123	235032.816791	56.031015
2782.723120	234818.085794	56.036020
2781.883319	234621.183279	56.041025
2781.227417	234406.758729	56.046029
2780.732721	234196.612392	56.051034
2779.909579	234014.757201	56.056039
2779.399765	233805.505290	56.061044
2778.790067	233602.890043	56.066049
2777.942050	233395.831460	56.071053
2777.441357	233189.762286	56.076058
2776.689875	232998.145288	56.081063
2776.124518	232788.140445	56.086068
2774.969519	232595.773338	56.091073
2774.671733	232393.085732	56.096077
2774.099180	232182.675940	56.101082
2773.346870	231989.202295	56.106087
2772.808251	231777.718588	56.111092
2772.076960	231578.207810	56.116097
2771.258749	231374.509907	56.121101
2770.780126	231170.911434	56.126106
2769.869817	230978.432459	56.131111
2769.111316	230768.589981	56.136116
2768.640374	230580.421765	56.141121
2768.229310	230377.654586	56.146125
2766.971653	230174.869170	56.151130
2766.273267	229988.469619	56.156135
2765.906938	229777.701578	56.161140
2764.985823	229589.072000	56.166145
2764.480832	229390.243047	56.171149
2764.165388	229185.426427	56.176154
2763.095925	228997.636369	56.181159
2762.577575	228792.012548	56.186164
2762.165740	228597.371802	56.191169
2761.773136	228386.178349	56.196173
2760.872130	228185.377883	56.201178
2760.010249	227992.617532	56.206183
2759.567222	227777.945300	56.211188
2758.805277	227588.530934	56.216193
2757.992227	227380.309117	56.221197
2757.378493	227182.113455	56.226202
2756.551286	226984.664978	56.231207
2756.167772	226779.864779	56.236212
2755.951619	226581.913072	56.241217
2754.699686	226379.466509	56.246221
2754.208892	226177.447286	56.251226
2753.634480	225987.013800	56.256231
2753.363805	225769.149443	56.261236
2752.487138	225564.914070	56.266241
2751.650977	225355.300564	56.271245
2751.188131	225154.361480	56.276250
2750.644483	224946.905032	56.281255
2749.871891	224738.492411	56.286260
2748.845252	224536.345657	56.291265
2748.021072	224323.715826	56.296269
2747.668256	224127.179233	56.301274
2746.489672	223926.954870	56.306279
2746.284882	223725.036418	56.311284
2745.298103	223517.895699	56.316289
2744.514900	223322.473122	56.321293
2743.940922	223125.172032	56.326298
2743.330573	222930.779636	56.331303
2742.827531	222731.049596	56.336308
2742.131942	222538.135620	56.341313
2741.730459	222333.604053	56.346317
2741.093650	222126.487945	56.351322
2740.471862	221933.729267	56.356327
2739.969347	221728.820674	56.361332
2739.208545	221519.014389	56.366337
2738.237408	221312.169835	56.371341
2737.876459	221102.224979	56.376346
2736.631100	220905.214107	56.381351
2736.407616	220706.501598	56.386356
2735.808541	220505.786911	56.391361
2735.077241	220295.979336	56.396365
2734.596413	220098.505777	56.401370
2733.560250	219898.422053	56.406375
2733.062793	219687.789919	56.411380
2732.339217	219475.743049	56.416385
2731.795653	219280.891135	56.421389
2731.151415	219080.722086	56.426394
2730.481941	218870.997863	56.431399
2729.755770	218667.940638	56.436404
2729.385649	218465.654982	56.441409
2728.632819	218264.639788	56.446413
2727.967870	218058.774147	56.451418
2727.157252	217860.429634	56.456423
2726.485066	217641.646259	56.461428
2725.820986	217431.339828	56.466433
2725.139039	217232.391141	56.471437
2724.529589	217032.400480	56.476442
2723.735100	216820.347190	56.481447
2723.317948	216610.118645	56.486452
2722.580855	216409.220765	56.491457
2721.796769	216214.758971	56.496461
2721.423885	216007.274658	56.501466
2720.581776	215803.263875	56.506471
2719.918763	215595.801296	56.511476
2719.451922	215394.227108	56.516481
2718.779990	215182.681277	56.521485
2718.287865	214977.917426	56.526490
2717.452100	214772.508553	56.531495
2716.899104	214556.223523	56.536500
2716.141337	214351.503640	56.541505
2715.478731	214147.240256	56.546509
2714.818168	213928.568598	56.551514
2714.003386	213726.621716	56.556519
2713.351802	213512.595854	56.561524
2712.505828	213314.537305	56.566529
2711.981102	213101.994609	56.571533
2711.292717	212895.957186	56.576538
2710.450156	212701.552932	56.581543
2709.993802	212492.959835	56.586548
2709.309304	212289.227493	56.591553
2708.552997	212082.376060	56.596557
2708.396603	211872.680998	56.601562
2707.413558	211664.797659	56.606567
2706.709281	211459.620065	56.611572
2705.984129	211254.637349	56.616577
2705.214364	211048.720494	56.621581
2704.578207	210841.586721	56.626586
2703.822806	210644.731100	56.631591
2703.360347	210431.601817	56.636596
2702.415022	210235.172113	56.641601
2701.424411	210028.771712	56.646605
2701.348984	209826.579852	56.651610
2700.453319	209630.385993	56.656615
2699.725837	209435.286129	56.661620
2699.348538	209228.969389	56.666625
2698.588825	209027.384888	56.671629
2697.731613	208822.634636	56.676634
2697.008812	208625.500189	56.681639
2696.618451	208418.870033	56.686644
2695.989982	208219.660116	56.691649
2695.255697	208031.769402	56.696653
2694.975840	207813.020175	56.701658
2693.945204	207612.666864	56.706663
2693.490890	207408.646597	56.711668
2693.121936	207200.413560	56.716673
2692.168541	206998.739159	56.721677
2691.606238	206784.823753	56.726682
2690.644040	206586.448420	56.731687
2690.248662	206368.600887	56.736692
2689.558977	206167.892932	56.741697
2688.928539	205961.041949	56.746701
2688.217495	205749.330107	56.751706
2687.705159	205549.016137	56.756711
2686.874761	205337.719210	56.761716
2686.366013	205135.751611	56.766721
2685.646563	204929.885574	56.771725
2685.226384	204714.440676	56.776730
2684.399979	204508.440354	56.781735
2683.856747	204301.530503	56.786740
2682.991481	204092.814357	56.791745
2681.765784	203888.928449	56.796749
2681.621977	203674.716274	56.801754
2681.154793	203471.424356	56.806759
2680.258747	203253.425966	56.811764
2679.565684	203059.194187	56.816769
2679.009394	202857.649334	56.821773
2678.585742	202646.883228	56.826778
2677.515309	202441.679842	56.831783
2676.776453	202226.332967	56.836788
2676.218003	202026.827580	56.841793
2675.367887	201823.538617	56.846797
2675.079714	201612.462231	56.851802
2674.474753	201412.406469	56.856807
2673.588643	201195.152577	56.861812
2672.924282	200995.845821	56.866817
2672.501933	200786.919023	56.871821
2671.797866	200577.375918	56.876826
2670.727470	200367.815297	56.881831
2670.211254	200168.488067	56.886836
2669.875064	199963.559291	56.891841
2668.883591	199754.510263	56.896845
2668.345270	199540.287375	56.901850
2667.990331	199337.374537	56.906855
2667.302411	199133.586271	56.911860
2666.404276	198920.186363	56.916865
2665.596431	198712.053943	56.921869
2665.252904	198500.667490	56.926874
2664.504645	198300.327730	56.931879
2663.873185	198084.572943	56.936884
2663.297258	197878.341234	56.941889
2662.093741	197680.773631	56.946893
2661.840232	197464.388867	56.951898
2661.028545	197257.102595	56.956903
2660.341460	197048.346777	56.961908
2659.307373	196848.681317	56.966913
2658.947499	196650.156820	56.971917
2658.594159	196439.849042	56.976922
2657.402536	196239.421949	56.981927
2657.154662	196031.491333	56.986932
2656.349740	195827.836159	56.991937
2655.475739	195622.004133	56.996941
2655.167433	195418.908114	57.001946
2654.197246	195211.120694	57.006951
2653.670503	195003.989144	57.011956
2653.029731	194812.501839	57.016961
2652.545416	194604.576286	57.021965
2652.105255	194390.091668	57.026970
2651.300379	194183.910934	57.031975
2650.564731	193972.783156	57.036980
2649.994985	193765.472611	57.041985
2649.053342	193558.501770	57.046989
2648.574877	193347.399489	57.051994
2647.531929	193143.729165	57.056999
2647.069113	192935.323590	57.062004
2646.350737	192743.322049	57.067009
2645.727834	192539.282278	57.072013
2645.508791	192319.147636	57.077018
2644.547531	192124.362340	57.082023
2643.812646	191915.291643	57.087028
2643.165673	191700.609597	57.092033
2642.673045	191494.670441	57.097037
2642.008047	191286.571050	57.102042
2641.271395	191081.461144	57.107047
2640.549446	190874.822987	57.112052
2639.998828	190662.496758	57.117057
2639.065442	190465.143584	57.122061
2638.708101	190237.762609	57.127066
2638.124421	190042.238767	57.132071
2637.499058	189833.833984	57.137076
2636.673906	189631.517855	57.142081
2635.690434	189420.856045	57.147085
2635.486029	189204.982617	57.152090
2634.545960	189005.244628	57.157095
2634.292072	188795.220627	57.162100
2633.419656	188583.488949	57.167105
2632.510508	188383.430617	57.172109
2632.172863	188162.697587	57.177114
2631.717063	187960.113781	57.182119
2630.813766	187746.813175	57.187124
2630.139760	187537.395687	57.192129
2629.695829	187335.067151	57.197133
2628.759595	187118.912123	57.202138
2627.970282	186911.411327	57.207143
2627.581229	186699.471639	57.212148
2626.828139	186487.374328	57.217153
2625.629658	186284.024953	57.222157
2625.410007	186074.325806	57.227162
2624.585400	185868.183817	57.232167
2623.966023	185659.631260	57.237172
2623.331378	185457.252121	57.242177
2622.962089	185248.699979	57.247181
2622.146955	185033.260703	57.252186
2621.692834	184838.259703	57.257191
2620.865740	184624.618006	57.262196
2620.321621	184410.779825	57.267201
2619.645582	184196.378377	57.272205
2619.245870	183986.819159	57.277210
2618.271118	183773.866405	57.282215
2617.631206	183557.528651	57.287220
2617.074995	183343.188625	57.292225
2615.849253	183136.690142	57.297229
2615.633317	182923.290466	57.302234
2614.744990	182731.496805	57.307239
2614.082406	182521.897080	57.312244
2613.560205	182312.606849	57.317249
2612.718433	182110.619104	57.322253
2612.094530	181892.696842	57.327258
2611.279382	181688.086351	57.332263
2610.581309	181476.372882	57.337268
2609.848874	181274.002773	57.342273
2609.175057	181067.019495	57.347277
2608.807192	180863.308757	57.352282
2607.946507	180666.787756	57.357287
2607.549256	180462.371218	57.362292
2607.141311	180255.311527	57.367297
2606.074156	180040.534368	57.372301
2605.555333	179833.099952	57.377306
2605.093829	179621.129111	57.382311
2604.127749	179413.449596	57.387316
2603.487439	179202.246925	57.392321
2602.839640	178998.627537	57.397325
2602.421788	178782.736220	57.402330
2601.494030	178585.510365	57.407335
2600.817710	178376.746979	57.412340
2600.191605	178166.043283	57.417345
2599.392280	177968.380210	57.422349
2598.748198	177749.744432	57.427354
2598.024406	177551.995033	57.432359
2597.263317	177343.542754	57.437364
2596.741505	177138.195271	57.442369
2596.168652	176949.875260	57.447373
2595.571340	176732.025988	57.452378
2594.756800	176527.312988	57.457383
2594.235599	176329.855264	57.462388
2593.467788	176116.551516	57.467393
2592.614035	175906.569414	57.472397
2592.268116	175704.889653	57.477402
2591.566978	175503.038231	57.482407
2590.685864	175291.817162	57.487412
2590.110259	175085.102061	57.492417
2589.554150	174887.173488	57.497421
2589.065820	174673.247901	57.502426
2588.076184	174479.485386	57.507431
2587.587615	174275.355177	57.512436
2587.013973	174062.552830	57.517441
2586.011578	173857.997416	57.522445
2585.338149	173653.174699	57.527450
2584.741310	173446.013461	57.532455
2584.453423	173254.447610	57.537460
2583.658713	173044.318326	57.542465
2582.953179	172843.561885	57.547469
2582.171412	172632.682352	57.552474
2581.510219	172428.830517	57.557479
2580.965856	172215.689947	57.562484
2580.522489	172017.248917	57.567489
2579.358456	171820.245719	57.572493
2578.871463	171610.024377	57.577498
2578.284267	171402.757781	57.582503
2577.917275	171202.312090	57.587508
2577.383961	170990.677038	57.592513
2576.789154	170786.161855	57.597517
2575.938920	170565.397415	57.602522
2575.271653	170368.297341	57.607527
2573.968955	170157.233826	57.612532
2573.818766	169944.272015	57.617537
2572.953976	169751.250391	57.622541
2572.564104	169530.228115	57.627546
2571.857827	169327.569498	57.632551
2570.968245	169120.630006	57.637556
2570.298284	168911.329664	57.642561
2569.761157	168714.954952	57.647565
2569.310492	168496.873065	57.652570
2568.452670	168290.835887	57.657575
2567.980520	168088.985990	57.662580
2567.189675	167882.609774	57.667585
2566.336758	167668.538436	57.672589
2565.654776	167459.909193	57.677594
2564.976992	167258.744817	57.682599
2564.109723	167058.908580	57.687604
2563.656942	166849.725017	57.692609
2563.069078	166656.166496	57.697613
2562.679858	166440.502710	57.702618
2561.780144	166242.748633	57.707623
2561.111805	166043.013422	57.712628
2560.565672	165823.932081	57.717633
2559.529252	165626.075771	57.722637
2559.221369	165414.690164	57.727642
2558.750283	165213.809163	57.732647
2557.955438	165012.967841	57.737652
2557.017871	164797.260580	57.742657
2556.359199	164590.461914	57.747661
2556.047468	164384.296042	57.752666
2555.328026	164186.053876	57.757671
2554.280002	163975.709271	57.762676
2554.039116	163763.953744	57.767681
2553.199756	163499.985252	57.772685
2552.792200	163292.696355	57.777690
2552.212274	163077.158663	57.782695
2551.285389	162873.603578	57.787700
2550.906604	162653.510100	57.792705
2550.249847	162452.660913	57.797709
2549.755364	162233.287618	57.802714
2548.828944	162027.804615	57.807719
2547.954627	161819.377525	57.812724
2547.519102	161603.634999	57.817729
2546.699942	161392.035805	57.822733
2545.898834	161176.328356	57.827738
2545.567535	160981.029981	57.832743
2544.819026	160766.651634	57.837748
2544.510898	160555.090823	57.842753
2543.552446	160346.088090	57.847757
2542.932432	160132.341597	57.852762
2542.036495	159919.695352	57.857767
2541.379696	159713.343824	57.862772
2541.241360	159496.982119	57.867777
2539.937352	159291.015328	57.872781
2539.479161	159075.762110	57.877786
2538.894637	158876.726889	57.882791
2538.035058	158663.675633	57.887796
2537.505140	158452.874494	57.892801
2536.658500	158244.095337	57.897805
2536.208826	158027.893730	57.902810
2535.576019	157826.062583	57.907815
2534.721319	157621.356549	57.912820
2534.254288	157405.720921	57.917825
2533.637234	157200.763588	57.922829
2533.031529	156988.661219	57.927834
2532.061007	156779.262166	57.932839
2531.498227	156566.812350	57.937844
2530.948876	156356.624508	57.942849
2529.782200	156153.108020	57.947853
2529.403721	155932.687768	57.952858
2528.864062	155737.972880	57.957863
2528.015747	155526.184945	57.962868
2527.616251	155313.132271	57.967873
2526.927757	155106.597063	57.972877
2526.001842	154902.528689	57.977882
2525.438794	154699.954857	57.982887
2524.618824	154504.910102	57.987892
2524.060952	154290.109324	57.992897
2523.458975	154079.982010	57.997901
2522.801474	153863.572671	58.002906
2522.171482	153660.113181	58.007911
2521.223471	153458.192542	58.012916
2520.959310	153247.953330	58.017921
2520.364856	153040.894711	58.022925
2519.761758	152829.987315	58.027930
2518.903523	152622.668035	58.032935
2518.517241	152417.906385	58.037940
2517.919682	152200.506864	58.042945
2517.052762	151992.557354	58.047949
2516.252473	151771.557527	58.052954
2515.476616	151573.192712	58.057959
2514.911613	151368.021011	58.062964
2514.253535	151149.430502	58.067969
2513.461911	150946.725021	58.072973
2512.734044	150734.694119	58.077978
2512.329958	150538.742395	58.082983
2511.545667	150327.460259	58.087988
2510.758118	150111.706105	58.092993
2510.166516	149913.601740	58.097997
2509.526537	149712.837192	58.103002
2509.156582	149529.227326	58.108007
2508.279707	149322.656269	58.113012
2507.669630	149096.064829	58.118017
2506.694265	148884.301267	58.123021
2506.191464	148677.242919	58.128026
2505.700453	148466.765230	58.133031
2504.821603	148261.345112	58.138036
2504.201583	148041.689182	58.143041
2503.532420	147840.000427	58.148045
2503.161066	147627.158101	58.153050
2502.284938	147418.273408	58.158055
2501.248034	147223.865474	58.163060
2500.377917	147012.173843	58.168065
2499.881003	146815.077528	58.173069
2499.396012	146614.358605	58.178074
2498.920541	146406.751446	58.183079
2498.032697	146210.648569	58.188084
2497.629643	145996.907173	58.193089
2496.726158	145798.153299	58.198093
2496.185342	145597.297181	58.203098
2495.442345	145392.051983	58.208103
2494.916146	145191.030939	58.213108
2494.345389	144985.964423	58.218113
2493.736674	144786.941482	58.223117
2493.298548	144576.150816	58.228122
2492.354875	144364.272601	58.233127
2491.403046	144172.297175	58.238132
2490.908236	143951.366367	58.243137
2490.256655	143753.297175	58.248141
2489.584506	143541.203628	58.253146
2489.270159	143339.995745	58.258151
2488.540989	143140.240002	58.263156
2488.128628	142921.832191	58.268161
2487.333611	142717.032217	58.273165
2486.250146	142509.903139	58.278170
2485.592599	142300.204705	58.283175
2484.977759	142102.381719	58.288180
2484.575341	141880.231251	58.293185
2483.791455	141692.501363	58.298189
2482.969525	141476.430528	58.303194
2482.599470	141263.631373	58.308199
2481.828440	141074.645321	58.313204
2481.009619	140858.908741	58.318209
2480.263087	140649.769417	58.323213
2479.819461	140437.991492	58.328218
2479.356102	140232.266205	58.333223
2478.329139	140040.697043	58.338228
2477.921300	139828.689011	58.343233
2477.325967	139627.740726	58.348237
2476.380524	139412.479249	58.353242
2475.805963	139208.315962	58.358247
2475.084823	139008.459028	58.363252
2474.488432	138792.193770	58.368257
2473.718615	138590.162031	58.373261
2473.182482	138384.283070	58.378266
2472.720885	138176.564186	58.383271
2471.838598	137974.249532	58.388276
2471.666140	137755.853684	58.393281
2470.731682	137552.266982	58.398285
2469.942692	137344.809094	58.403290
2469.571191	137134.910718	58.408295
2468.646768	136929.954614	58.413300
2468.143109	136717.590067	58.418305
2467.459048	136504.938041	58.423309
2466.734052	136294.695149	58.428314
2466.106416	136084.425625	58.433319
2465.105149	135884.862861	58.438324
2464.622605	135672.540643	58.443329
2463.844939	135463.684102	58.448333
2463.540247	135253.636145	58.453338
2462.589294	135045.026039	58.458343
2461.876188	134840.038372	58.463348
2461.428607	134639.405486	58.468353
2460.415281	134432.448429	58.473357
2460.051271	134221.299440	58.478362
2459.196437	134005.161197	58.483367
2458.669745	133810.199557	58.488372
2458.099675	133586.206860	58.493377
2457.357043	133386.467855	58.498381
2456.788980	133177.645398	58.503386
2456.242699	132966.572611	58.508391
2455.690151	132763.746434	58.513396
2455.213888	132553.275326	58.518401
2454.436385	132345.533756	58.523405
2453.376438	132132.757501	58.528410
2453.082788	131906.663632	58.533415
2452.540413	131705.393055	58.538420
2451.881420	131481.900932	58.543425
2451.156740	131270.716563	58.548429
2450.344926	131049.119283	58.553434
2449.820507	130836.979165	58.558439
2448.953990	130631.766526	58.563444
2448.558570	130406.158039	58.568449
2447.626001	130206.916048	58.573453
2446.773722	129985.803506	58.578458
2446.369129	129770.972423	58.583463
2445.497855	129563.596411	58.588468
2444.771545	129358.713790	58.593473
2444.275676	129146.658130	58.598477
2443.726593	128934.917341	58.603482
2442.738715	128725.419578	58.608487
2442.235969	128515.643275	58.613492
2442.095646	128301.378555	58.618497
2440.773984	128096.929829	58.623501
2440.241099	127883.264002	58.628506
2439.867394	127664.342022	58.633511
2439.098910	127455.657312	58.638516
2438.477971	127248.678022	58.643521
2437.613142	127034.144282	58.648525
2437.086525	126816.027993	58.653530
2436.391919	126609.001701	58.658535
2435.329002	126396.599837	58.663540
2435.143607	126184.771692	58.668545
2434.152784	125979.854478	58.673549
2433.787593	125763.130651	58.678554
2433.286338	125546.773003	58.683559
2432.741205	125342.945571	58.688564
2432.004097	125130.717811	58.693569
2431.220530	124909.838268	58.698573
2430.598963	124692.592165	58.703578
2429.996309	124479.319572	58.708583
2429.188890	124268.252627	58.713588
2428.660267	124050.108038	58.718593
2427.981693	123832.052483	58.723597
2426.939102	123607.173809	58.728602
2426.811284	123399.739300	58.733607
2425.917427	123194.827823	58.738612
2425.172935	122973.157979	58.743617
2424.120711	122752.249855	58.748621
2423.663294	122539.185517	58.753626
2422.986430	122332.392346	58.758631
2422.432316	122130.965195	58.763636
2422.071764	121922.969557	58.768641
2421.476983	121711.647815	58.773645
2420.706615	121491.594311	58.778650
2420.113488	121274.015925	58.783655
2419.278107	121063.397768	58.788660
2418.420649	120847.972552	58.793665
2417.768088	120630.129559	58.798669
2417.057636	120420.334743	58.803674
2416.320310	120197.315703	58.808679
2415.681677	120001.047735	58.813684
2415.382332	119786.926683	58.818689
2414.637709	119576.236223	58.823693
2414.066485	119366.929280	58.828698
2413.388997	119141.103829	58.833703
2412.589900	118943.967797	58.838708
2411.595875	118723.515893	58.843713
2411.294289	118510.929207	58.848717
2410.584786	118295.374599	58.853722
2410.000587	118086.943337	58.858727
2409.123811	117874.554629	58.863732
2408.965724	117665.367286	58.868737
2408.029167	117447.595914	58.873741
2407.270035	117225.723017	58.878746
2407.175157	117008.589985	58.883751
2406.463210	116797.409118	58.888756
2405.542537	116576.932168	58.893761
2404.945237	116366.441250	58.898765
2404.096084	116140.491516	58.903770
2403.696255	115925.002869	58.908775
2402.831387	115714.724772	58.913780
2402.362628	115484.505896	58.918785
2401.626416	115273.132007	58.923789
2400.967202	115057.380807	58.928794
2400.553053	114838.520577	58.933799
2399.412418	114625.857913	58.938804
2398.576630	114391.016658	58.943809
2398.012310	114180.798820	58.948813
2397.667869	113962.969664	58.953818
2397.139128	113742.131468	58.958823
2396.234577	113540.001684	58.963828
2395.715689	113309.264719	58.968833
2395.173282	113093.467352	58.973837
2394.386956	112878.446724	58.978842
2393.999030	112650.633545	58.983847
2392.736147	112444.545678	58.988852
2392.544476	112199.747590	58.993857
2391.570840	112000.744605	58.998861
2391.001682	111781.611902	59.003866
2390.625032	111562.450607	59.008871
2389.746328	111343.821430	59.013876
2389.044400	111117.017651	59.018881
2388.471784	110894.364850	59.023885
2387.728444	110688.926285	59.028890
2387.436446	110463.199451	59.033895
2386.264333	110235.094882	59.038900
2385.761081	110019.007045	59.043905
2384.996470	109803.806542	59.048909
2384.123590	109573.915554	59.053914
2383.482144	109363.401612	59.058919
2383.041142	109156.500116	59.063924
2382.434444	108927.842120	59.068929
2381.904433	108709.682353	59.073933
2381.013375	108495.458888	59.078938
2380.333071	108271.730132	59.083943
2379.719096	108051.616134	59.088948
2378.849585	107833.619571	59.093953
2378.404263	107623.889058	59.098957
2377.621025	107406.263373	59.103962
2377.265179	107187.651828	59.108967
2376.504324	106975.635594	59.113972
2376.107324	106749.147570	59.118977
2375.405330	106529.486484	59.123981
2374.551477	106311.025292	59.128986
2373.883611	106085.449368	59.133991
2373.243966	105869.172590	59.138996
2372.513554	105641.802479	59.144001
2372.132974	105416.174606	59.149005
2371.406956	105198.464642	59.154010
2370.921898	104964.964861	59.159015
2369.893497	104750.155647	59.164020
2369.526857	104521.609191	59.169025
2368.982251	104298.707942	59.174029
2367.931513	104081.402271	59.179034
2367.313114	103858.700839	59.184039
2366.729168	103637.734353	59.189044
2366.099681	103404.881844	59.194049
2365.306270	103186.509485	59.199053
2364.476305	102968.976011	59.204058
2364.076756	102740.788186	59.209063
2363.212729	102527.222838	59.214068
2362.538001	102297.738030	59.219073
2362.227151	102075.004666	59.224077
2361.185938	101865.939468	59.229082
2360.636633	101636.434898	59.234087
2360.073314	101412.491816	59.239092
2359.284297	101190.667358	59.244097
2358.876283	100969.698058	59.249101
2358.101738	100751.668897	59.254106
2357.654591	100523.535601	59.259111
2356.879786	100312.811830	59.264116
2356.185093	100081.664643	59.269121
2355.658210	99858.358719	59.274125
2354.382380	99640.578065	59.279130
2353.952976	99410.042518	59.284135
2353.145201	99197.272630	59.289140
2352.763555	98969.626325	59.294145
2352.389886	98757.483043	59.299149
2351.518867	98535.849238	59.304154
2351.095724	98312.776512	59.309159
2350.122775	98095.121018	59.314164
2349.880497	97869.505865	59.319169
2348.898073	97638.010212	59.324173
2348.021453	97416.128080	59.329178
2347.595747	97182.544525	59.334183
2346.660949	96958.545004	59.339188
2346.330833	96731.236236	59.344193
2345.680050	96519.563559	59.349197
2344.764136	96293.937626	59.354202
2344.524516	96065.574703	59.359207
2343.378549	95847.467093	59.364212
2342.744726	95618.276957	59.369217
2342.291963	95393.125632	59.374221
2341.516085	95176.678142	59.379226
2340.792382	94948.270092	59.384231
2339.938191	94724.482837	59.389236
2339.445954	94509.632962	59.394241
2338.814600	94286.772331	59.399245
2338.030499	94069.658248	59.404250
2338.029692	93835.585309	59.409255
2336.968537	93620.104903	59.414260
2336.380745	93399.598878	59.419265
2335.669314	93171.460647	59.424269
2334.766331	92945.809199	59.429274
2334.393556	92721.769062	59.434279
2333.380767	92498.885304	59.439284
2333.046123	92279.770646	59.444289
2332.428086	92058.109615	59.449293
2331.726650	91840.572967	59.454298
2331.424070	91608.619433	59.459303
2330.304939	91380.779858	59.464308
2329.313479	91158.235946	59.469313
2329.197549	90931.231088	59.474317
2328.290984	90704.823155	59.479322
2327.798877	90477.958715	59.484327
2326.711034	90255.426544	59.489332
2326.327465	90039.017595	59.494337
2325.706083	89817.474754	59.499341
2324.976280	89599.108823	59.504346
2324.969365	89368.672738	59.509351
2323.932583	89145.921853	59.514356
2323.229806	88916.716766	59.519361
2322.508276	88685.843295	59.524365
2321.616950	88464.642309	59.529370
2320.962451	88230.637438	59.534375
2320.330321	88012.893244	59.539380
2319.605305	87795.482959	59.544385
2319.367800	87570.307469	59.549389
2318.214705	87347.732969	59.554394
2317.823268	87117.603645	59.559399
2317.120189	86897.694786	59.564404
2316.126083	86678.721850	59.569409
2315.475058	86457.687151	59.574413
2315.120330	86233.381022	59.579418
2314.682213	86009.439122	59.584423
2313.571625	85788.351076	59.589428
2312.867677	85568.551063	59.594433
2312.729774	85342.926693	59.599437
2311.791083	85124.670832	59.604442
2311.082149	84889.880541	59.609447
2310.575519	84670.743089	59.614452
2309.556279	84449.204382	59.619457
2309.195244	84230.732966	59.624461
2308.476030	84005.278348	59.629466
2308.016202	83772.286438	59.634471
2307.240935	83555.307520	59.639476
2306.418579	83321.313198	59.644481
2306.103390	83109.235247	59.649485
2305.004690	82886.565574	59.654490
2304.644554	82656.732985	59.659495
2304.009029	82431.129782	59.664500
2303.476622	82204.726721	59.669505
2302.661834	81974.980027	59.674509
2301.739660	81753.143671	59.679514
2301.323432	81527.471041	59.684519
2300.431494	81318.126537	59.689524
2299.711199	81091.898398	59.694529
2299.174803	80865.935082	59.699533
2298.410211	80654.194063	59.704538
2298.069730	80423.451238	59.709543
2297.259497	80205.042219	59.714548
2296.310336	79978.418852	59.719553
2296.000889	79752.057736	59.724557
2294.908293	79531.577571	59.729562
2294.732962	79302.563776	59.734567
2293.853185	79091.173841	59.739572
2293.141210	78866.825424	59.744577
2292.887984	78633.636236	59.749581
2292.131308	78410.598966	59.754586
2291.569600	78182.945280	59.759591
2290.671754	77964.504138	59.764596
2290.006841	77740.952635	59.769601
2289.429709	77508.486603	59.774605
2288.440018	77279.459719	59.779610
2288.402141	77059.662530	59.784615
2287.466445	76840.333257	59.789620
2286.600424	76611.953236	59.794625
2286.438394	76387.886884	59.799629
2285.211931	76166.095457	59.804634
2284.753942	75941.149531	59.809639
2284.053150	75713.741833	59.814644
2283.414361	75490.153828	59.819649
2282.829327	75256.561577	59.824653
2282.127126	75038.203135	59.829658
2281.757796	74807.407676	59.834663
2280.892086	74589.910006	59.839668
2280.348373	74361.409175	59.844673
2279.919064	74123.750474	59.849677
2278.535990	73906.887098	59.854682
2278.247079	73675.832083	59.859687
2277.512030	73452.776092	59.864692
2276.619376	73217.254276	59.869697
2276.003099	72992.841472	59.874701
2275.076841	72781.309137	59.879706
2274.876910	72547.668252	59.884711
2274.070509	72331.877129	59.889716
2273.533980	72108.842649	59.894721
2273.045183	71878.030147	59.899725
2272.208569	71664.176864	59.904730
2271.843733	71431.024998	59.909735
2271.103783	71204.187717	59.914740
2270.514907	70970.265955	59.919745
2269.844769	70739.799508	59.924750
2268.930571	70520.105071	59.929754
2268.423115	70277.500341	59.934759
2267.536568	70065.426871	59.939764
2266.891938	69834.561543	59.944769
2266.625345	69599.205026	59.949774
2265.883075	69382.207033	59.954778
2265.223019	69145.911223	59.959783
2264.641578	68920.202519	59.964788
2263.789483	68686.051919	59.969793
2263.166006	68453.248632	59.974798
2262.288281	68239.153996	59.979802
2261.730367	68001.633377	59.984807
2260.968058	67776.834265	59.989812
2260.185602	67551.242917	59.994817
2259.752160	67328.765553	59.999822
2258.822384	67095.216372	60.004826
2258.217633	66869.174079	60.009831
2257.452076	66641.817279	60.014836
2256.889542	66418.230838	60.019841
2256.241959	66196.959378	60.024846
2255.574080	65979.506143	60.029850
2254.851116	65749.667359	60.034855
2254.063374	65528.397288	60.039860
2253.266135	65305.864704	60.044865
2252.993421	65086.743990	60.049870
2251.928466	64860.763355	60.054874
2251.313756	64641.730454	60.059879
2250.519517	64427.211941	60.064884
2250.184462	64191.678481	60.069889
2249.682698	63978.195114	60.074894
2248.554635	63765.190241	60.079898
2248.031515	63539.598333	60.084903
2247.672520	63320.305695	60.089908
2246.494332	63098.707670	60.094913
2246.080112	62886.045795	60.099918
2245.226266	62671.068893	60.104922
2244.812673	62457.465086	60.109927
2244.080340	62234.422902	60.114932
2243.610027	62012.174397	60.119937
2243.117295	61791.951844	60.124942
2241.903130	61576.078931	60.129946
2241.862842	61350.645355	60.134951
2240.986954	61122.136988	60.139956
2240.173095	60905.521285	60.144961
2239.824836	60686.925342	60.149966
2239.048862	60469.298808	60.154970
2238.395979	60238.068705	60.159975
2237.557624	60022.267937	60.164980
2236.735086	59795.666524	60.169985
2236.410596	59571.771270	60.174990
2235.484132	59361.082119	60.179994
2235.076847	59141.747497	60.184999
2234.474727	58915.074296	60.190004
2233.637622	58693.043456	60.195009
2232.851460	58470.253847	60.200014
2232.186949	58255.452442	60.205018
2231.469961	58040.617527	60.210023
2230.946745	57822.832927	60.215028
2230.042507	57603.595233	60.220033
2229.776940	57378.153400	60.225038
2228.908299	57165.128275	60.230042
2228.315972	56935.575310	60.235047
2227.752133	56712.974080	60.240052
2226.949098	56503.291528	60.245057
2226.395929	56274.557110	60.250062
2225.622477	56063.286095	60.255066
2224.954787	55840.221315	60.260071
2224.420534	55625.432930	60.265076
2223.468657	55400.798197	60.270081
2223.298577	55179.153089	60.275086
2222.147071	54969.517972	60.280090
2221.692732	54747.663667	60.285095
2221.177043	54531.707900	60.290100
2220.168911	54309.677762	60.295105
2219.583583	54086.513652	60.300110
2218.957064	53877.538775	60.305114
2218.357117	53657.119499	60.310119
2217.723219	53443.679429	60.315124
2216.920322	53223.259627	60.320129
2216.533369	53005.814257	60.325134
2215.490294	52790.450081	60.330138
2214.865473	52569.547979	60.335143
2214.225161	52343.939531	60.340148
2213.654431	52126.894570	60.345153
2213.148033	51910.705812	60.350158
2212.111984	51701.029922	60.355162
2211.939201	51483.524555	60.360167
2210.977387	51267.855542	60.365172
2210.101070	51063.565859	60.370177
2209.774894	50836.746247	60.375182
2209.010624	50631.791921	60.380186
2208.289038	50407.891120	60.385191
2207.782283	50191.036502	60.390196
2206.808880	49979.829957	60.395201
2206.400897	49756.115338	60.400206
2205.518882	49542.982221	60.405210
2205.239152	49325.975516	60.410215
2204.473303	49102.173994	60.415220
2203.573621	48890.158743	60.420225
2203.317004	48666.949417	60.425230
2202.507773	48458.803467	60.430234
2201.767230	48241.152296	60.435239
2201.125375	48026.778112	60.440244
2200.301318	47811.688857	60.445249
2199.665440	47597.040537	60.450254
2198.728163	47384.438689	60.455258
2198.308606	47166.417637	60.460263
2197.687144	46951.237102	60.465268
2196.699280	46741.418852	60.470273
2196.373238	46526.373768	60.475278
2195.509858	46318.321668	60.480282
2194.729598	46114.585956	60.485287
2194.407279	45893.911361	60.490292
2193.959570	45687.894715	60.495297
2193.255028	45466.511183	60.500302
2192.295846	45253.372346	60.505306
2191.526128	45041.841266	60.510311
2190.755676	44827.675027	60.515316
2189.593420	44621.075793	60.520321
2189.551763	44409.737320	60.525326
2188.650189	44207.042463	60.530330
2188.149539	43999.254476	60.535335
2187.354057	43788.612402	60.540340
2186.528664	43588.860263	60.545345
2186.275838	43366.881367	60.550350
2185.496860	43173.205157	60.555354
2184.867203	42965.554343	60.560359
2184.422952	42755.618581	60.565364
2183.449239	42548.963434	60.570369
2182.996339	42340.245295	60.575374
2181.830130	42136.003753	60.580378
2181.539516	41925.595136	60.585383
2181.079009	41717.774333	60.590388
2180.434640	41523.690447	60.595393
2179.895707	41308.231181	60.600398
2178.623359	41095.809661	60.605402
2178.066972	40881.765672	60.610407
2177.668319	40689.192176	60.615412
2176.962396	40476.960382	60.620417
2176.104722	40264.262011	60.625422
2175.463208	40063.395788	60.630426
2174.656763	39853.233474	60.635431
2173.891939	39653.895128	60.640436
2173.189006	39459.709480	60.645441
2172.827475	39252.242709	60.650446
2171.827526	39044.179405	60.655450
2171.170794	38848.254389	60.660455
2170.843727	38639.292506	60.665460
2170.065485	38456.570958	60.670465
2169.508135	38237.801852	60.675470
2168.670653	38039.048787	60.680474
2168.244121	37831.181241	60.685479
2167.384673	37630.043134	60.690484
2166.603350	37436.376727	60.695489
2165.950498	37240.259400	60.700494
2165.199162	37041.240387	60.705498
2164.545674	36836.708943	60.710503
2163.891085	36636.982253	60.715508
2163.288108	36443.575543	60.720513
2162.586803	36245.781400	60.725518
2161.797207	36045.297559	60.730522
2161.175693	35847.443275	60.735527
2160.508724	35659.621032	60.740532
2160.201731	35455.362757	60.745537
2159.548293	35252.682420	60.750542
2158.446350	35062.247358	60.755546
2158.098763	34871.304390	60.760551
2157.365776	34673.366253	60.765556
2156.494028	34471.589791	60.770561
2155.771664	34280.107707	60.775566
2155.311791	34085.287794	60.780570
2154.185226	33895.288747	60.785575
2153.753808	33707.444711	60.790580
2152.936513	33513.974629	60.795585
2152.360597	33315.970774	60.800590
2151.712599	33137.047615	60.805594
2150.713992	32944.145505	60.810599
2150.650495	32755.970955	60.815604
2149.850153	32568.147748	60.820609
2149.185546	32369.345915	60.825614
2148.520300	32179.029391	60.830618
2147.717788	31995.772064	60.835623
2146.779738	31807.566891	60.840628
2145.764258	31619.641621	60.845633
2145.219434	31440.312722	60.850638
2144.311792	31261.147628	60.855642
2143.421689	31077.953889	60.860647
2143.088488	30899.099786	60.865652
2142.163682	30737.830251	60.870657
2141.376514	30563.314990	60.875662
2140.650906	30403.191150	60.880666
2140.046865	30225.997447	60.885671
2139.185859	30068.243182	60.890676
2138.072831	29912.431211	60.895681
2137.422567	29743.957657	60.900686
2136.577548	29596.432899	60.905690
2135.650326	29448.292096	60.910695
2135.103971	29290.763995	60.915700
2134.008627	29152.652249	60.920705
2133.073657	29010.648498	60.925710
2132.684114	28874.656430	60.930714
2131.613629	28733.961081	60.935719
2130.657567	28602.661918	60.940724
2129.937623	28477.870302	60.945729
2129.568724	28340.658147	60.950734
2128.533484	28224.833814	60.955738
2127.726263	28103.375082	60.960743
2127.181887	27973.573420	60.965748
2126.571812	27863.213690	60.970753
2125.743855	27740.648750	60.975758
2125.219468	27618.752225	60.980762
2124.558947	27504.734597	60.985767
2124.026958	27380.596161	60.990772
2123.200067	27258.947813	60.995777
2122.420564	27136.223355	61.000782
2122.039867	27022.559662	61.005786
2120.843253	26911.026194	61.010791
2120.601902	26790.253686	61.015796
2119.714424	26673.451773	61.020801
2118.953585	26561.284451	61.025806
2118.392803	26460.159109	61.030810
2117.718953	26337.607983	61.035815
2117.299941	26228.829306	61.040820
2116.752567	26123.672593	61.045825
2116.282924	25998.994620	61.050830
2115.324540	25892.050904	61.055834
2114.813811	25767.681374	61.060839
2114.435404	25646.832539	61.065844
2113.330199	25540.214587	61.070849
2112.824513	25435.126837	61.075854
2112.075948	25322.575238	61.080858
2111.517246	25195.822285	61.085863
2111.058907	25087.217097	61.090868
2110.093603	24970.794496	61.095873
2110.012100	24850.665091	61.100878
2109.176081	24737.987728	61.105882
2108.389325	24621.386907	61.110887
2107.904327	24499.378973	61.115892
2107.056534	24396.427789	61.120897
2106.408895	24276.186396	61.125902
2105.839517	24160.018812	61.130906
2105.131921	24042.403519	61.135911
2104.670609	23921.446577	61.140916
2103.772600	23815.772272	61.145921
2103.379628	23692.021660	61.150926
2102.676628	23576.849290	61.155930
2101.970871	23464.610366	61.160935
2101.173128	23343.454534	61.165940
2100.757034	23241.611838	61.170945
2100.036520	23117.960296	61.175950
2099.263242	23001.053290	61.180954
2098.393303	22883.567854	61.185959
2098.035251	22777.016393	61.190964
2097.120052	22659.918834	61.195969
2097.046421	22542.277972	61.200974
2096.305731	22429.208535	61.205978
2095.446421	22311.920684	61.210983
2094.937168	22181.070529	61.215988
2093.867342	22076.799541	61.220993
2093.498786	21965.538689	61.225998
2092.822119	21847.472772	61.231002
2091.847271	21730.089905	61.236007
2091.869468	21610.543283	61.241012
2090.893402	21501.900169	61.246017
2090.273016	21379.294882	61.251022
2089.580439	21259.711152	61.256026
2088.749417	21150.939259	61.261031
2088.176195	21029.465422	61.266036
2087.529435	20918.687980	61.271041
2086.978526	20800.955755	61.276046
2086.041078	20690.168407	61.281050
2085.884196	20574.805631	61.286055
2085.051007	20454.966070	61.291060
2084.334683	20338.251284	61.296065
2083.711121	20224.264730	61.301070
2083.110929	20113.037889	61.306074
2082.288449	19990.139127	61.311079
2081.703422	19878.467820	61.316084
2081.161790	19767.368746	61.321089
2080.357329	19639.085335	61.326094
2079.803223	19531.880635	61.331098
2079.100839	19412.860799	61.336103
2078.509634	19297.437358	61.341108
2077.648870	19181.917804	61.346113
2077.051724	19061.743906	61.351118
2076.245936	18940.519294	61.356122
2075.464765	18835.179487	61.361127
2074.950768	18724.166707	61.366132
2073.957063	18618.056437	61.371137
2073.719923	18505.467741	61.376142
2072.973664	18394.174827	61.381146
2072.356620	18281.664216	61.386151
2071.836526	18159.892705	61.391156
2071.091333	18048.253155	61.396161
2070.445162	17924.840543	61.401166
2069.884846	17813.978943	61.406170
2068.952327	17701.552972	61.411175
2068.383467	17582.378263	61.416180
2067.357656	17480.579174	61.421185
2066.992467	17368.729070	61.426190
2066.284973	17255.064806	61.431194
2065.574670	17143.161367	61.436199
2065.081315	17021.583964	61.441204
2064.111399	16926.466104	61.446209
2063.540669	16805.156854	61.451214
2062.666895	16700.128181	61.456218
2062.194651	16592.873451	61.461223
2061.599570	16484.702781	61.466228
2060.626531	16390.605395	61.471233
2060.302748	16277.355482	61.476238
2059.478600	16168.481388	61.481242
2058.605516	16059.324760	61.486247
2058.359161	15944.488495	61.491252
2057.664528	15840.190048	61.496257
2056.935282	15728.917273	61.501262
2056.163766	15623.523302	61.506266
2055.531009	15509.934568	61.511271
2054.989829	15411.471706	61.516276
2054.248673	15308.260446	61.521281
2053.753847	15195.866464	61.526286
2052.931632	15091.636338	61.531290
2051.937494	14987.702853	61.536295
2051.217197	14874.807720	61.541300
2050.582795	14773.133038	61.546305
2049.965231	14672.220757	61.551310
2049.559636	14579.149825	61.556314
2048.818195	14460.784325	61.561319
2048.196708	14363.953346	61.566324
2047.389507	14272.683068	61.571329
2047.005060	14164.470765	61.576334
2046.342409	14054.344308	61.581338
2045.446675	13955.254383	61.586343
2044.950669	13842.829926	61.591348
2044.270715	13750.180490	61.596353
2043.697746	13641.168484	61.601358
2042.835875	13532.080382	61.606362
2042.101100	13440.579230	61.611367
2041.392739	13325.323631	61.616372
2040.706027	13241.693282	61.621377
2040.373693	13139.614214	61.626382
2039.488033	13040.964041	61.631386
2038.503199	12942.482827	61.636391
2038.159979	12831.890973	61.641396
2037.409495	12744.220696	61.646401
2036.700001	12638.230113	61.651406
2036.066107	12539.028695	61.656410
2035.218323	12444.325784	61.661415
2034.248270	12348.518141	61.666420
2033.632219	12264.202777	61.671425
2032.944270	12173.756275	61.676430
2032.193733	12079.959735	61.681434
2031.251210	12007.514432	61.686439
2030.957563	11906.898435	61.691444
2030.273466	11821.895780	61.696449
2029.665523	11738.459540	61.701454
2028.971352	11651.846096	61.706458
2028.058859	11553.949304	61.711463
2027.643624	11461.215012	61.716468
2026.767528	11383.856127	61.721473
2026.112151	11289.768049	61.726478
2025.474856	11207.059825	61.731482
2024.382395	11136.113728	61.736487
2023.955864	11053.637626	61.741492
2023.051482	10975.397803	61.746497
2022.355050	10894.141518	61.751502
2021.866960	10815.521611	61.756506
2020.986377	10751.274012	61.761511
2020.639407	10662.704150	61.766516
2019.727807	10593.562502	61.771521
2019.198435	10514.972801	61.776526
2018.959870	10434.753741	61.781530
2018.110640	10351.796615	61.786535
2017.533664	10268.430620	61.791540
2016.860602	10201.838575	61.796545
2015.918278	10114.879973	61.801550
2015.458507	10037.163842	61.806554
2014.678357	9959.629938	61.811559
2014.258326	9882.364350	61.816564
2012.982770	9811.968368	61.821569
2012.362366	9735.659267	61.826574
2011.909815	9661.406091	61.831578
2010.875392	9592.739836	61.836583
2010.453108	9508.277292	61.841588
2009.985857	9441.925379	61.846593
2009.488366	9361.992968	61.851598
2008.839472	9283.231799	61.856602
2007.993218	9217.126838	61.861607
2006.806902	9138.542461	61.866612
2006.355838	9072.071658	61.871617
2005.794250	8997.362918	61.876622
2004.979987	8922.208257	61.881626
2004.488734	8857.865518	61.886631
2003.613786	8786.508579	61.891636
2002.968434	8722.435851	61.896641
2002.281623	8651.780658	61.901646
2001.674616	8574.010636	61.906650
2001.105896	8509.514823	61.911655
2000.499923	8435.814330	61.916660
1999.773242	8372.443960	61.921665
1998.881720	8309.991912	61.926670
1998.627626	8228.981953	61.931674
1997.136920	8177.187350	61.936679
1996.901790	8104.964477	61.941684
1996.149577	8043.420385	61.946689
1995.575306	7983.620996	61.951694
1994.950748	7917.486972	61.956698
1994.291020	7855.255244	61.961703
1994.128890	7800.605857	61.966708
1993.107301	7747.093024	61.971713
1992.656750	7676.169840	61.976718
1992.230918	7610.309358	61.981722
1991.131685	7553.171551	61.986727
1990.658975	7492.700068	61.991732
1990.060582	7418.220804	61.996737
1989.676822	7361.775617	62.001742
1988.851983	7287.796811	62.006746
1987.851837	7220.613169	62.011751
1987.176639	7146.863749	62.016756
1986.098482	7080.990026	62.021761
1985.772826	7022.177396	62.026766
1985.693902	6957.758837	62.031770
1984.512702	6894.861313	62.036775
1983.502286	6820.156981	62.041780
1983.207742	6764.229609	62.046785
1982.190214	6706.566964	62.051790
1981.701697	6636.963444	62.056794
1980.821978	6571.818557	62.061799
1980.050369	6498.542812	62.066804
1979.644766	6445.857848	62.071809
1978.748181	6386.908012	62.076814
1978.178893	6325.928864	62.081818
1977.673062	6265.077939	62.086823
1976.937672	6208.844389	62.091828
1976.030846	6156.062529	62.096833
1975.750900	6100.547492	62.101838
1975.041694	6038.415609	62.106842
1974.249761	5979.107648	62.111847
1973.947084	5918.658161	62.116852
1972.981501	5864.914855	62.121857
1972.497544	5807.835179	62.126862
1971.944260	5741.402124	62.131866
1970.903586	5687.060066	62.136871
1970.558035	5621.571100	62.141876
1969.890810	5564.635827	62.146881
1969.024267	5500.900748	62.151886
1968.582004	5436.930584	62.156890
1967.943675	5393.737473	62.161895
1967.332484	5319.433238	62.166900
1966.679704	5273.141311	62.171905
1965.715089	5213.011166	62.176910
1965.396721	5150.115019	62.181914
1964.298183	5099.762840	62.186919
1963.855380	5041.635261	62.191924
1963.063174	4984.094207	62.196929
1962.414503	4927.232585	62.201934
1962.089662	4866.031338	62.206938
1960.976965	4820.922031	62.211943
1960.574632	4755.874985	62.216948
1959.897553	4698.945398	62.221953
1959.400329	4645.165307	62.226958
1958.760083	4582.442557	62.231962
1957.975583	4527.022973	62.236967
1957.314033	4470.337097	62.241972
1956.482488	4414.956163	62.246977
1956.045099	4354.292306	62.251982
1955.318248	4297.805965	62.256986
1954.600042	4251.978776	62.261991
1954.268455	4182.904507	62.266996
1953.508835	4125.454698	62.272001
1952.620752	4072.020314	62.277006
1951.897451	4007.059068	62.282010
1951.330225	3956.260499	62.287015
1950.578947	3893.697117	62.292020
1949.977411	3849.266798	62.297025
1949.477120	3788.940985	62.302030
1949.008431	3728.863572	62.307034
1948.145785	3677.559201	62.312039
1947.434411	3608.313674	62.317044
1946.744425	3553.544457	62.322049
1946.086041	3505.273864	62.327054
1945.615408	3445.660081	62.332058
1944.933441	3385.005129	62.337063
1943.974236	3330.669085	62.342068
1943.314228	3272.381062	62.347073
1942.625755	3219.726473	62.352078
1942.324819	3164.258919	62.357082
1941.633035	3124.752948	62.362087
1940.861358	3056.934445	62.367092
1940.005906	2991.685571	62.372097
1939.314767	2943.097892	62.377102
1938.792187	2881.608989	62.382106
1938.007913	2840.402378	62.387111
1937.511914	2778.644702	62.392116
1936.683026	2732.550396	62.397121
1936.001250	2666.676823	62.402126
1935.590961	2615.058306	62.407130
1934.537829	2569.399949	62.412135
1934.049365	2514.994567	62.417140
1933.609021	2465.175471	62.422145
1932.720464	2412.660434	62.427150
1932.372253	2350.740726	62.432154
1931.353760	2301.383042	62.437159
1930.792942	2241.636268	62.442164
1930.177854	2197.877114	62.447169
1929.579191	2142.361326	62.452174
1929.210447	2088.444019	62.457178
1928.232037	2034.007802	62.462183
1927.611671	1972.017766	62.467188
1927.019833	1924.300935	62.472193
1926.138761	1863.637366	62.477198
1925.675434	1814.312273	62.482202
1924.838511	1760.507565	62.487207
1924.275253	1703.875919	62.492212
1923.714243	1659.464735	62.497217
1922.986582	1603.228634	62.502222
1922.211671	1544.851390	62.507226
1921.330086	1497.511578	62.512231
1920.732871	1434.863270	62.517236
1919.988301	1389.898510	62.522241
1919.355808	1338.221208	62.527246
1918.937331	1292.839874	62.532250
1917.896123	1242.434293	62.537255
1917.168574	1202.323342	62.542260
1916.677384	1151.524798	62.547265
1916.016087	1109.769705	62.552270
1915.396691	1053.272513	62.557274
1914.553307	1014.979141	62.562279
1913.835353	969.731523	62.567284
1913.122178	922.245412	62.572289
1912.464885	878.825742	62.577294
1912.064517	841.031820	62.582298
1911.399340	797.692497	62.587303
1910.701782	739.060973	62.592308
1909.747608	699.970684	62.597313
1908.817811	658.321811	62.602318
1908.796663	619.563033	62.607322
1907.626724	575.626381	62.612327
1907.089216	530.703163	62.617332
1906.334173	494.224928	62.622337
1905.453979	451.182564	62.627342
1905.091722	408.786684	62.632346
1904.302492	377.261291	62.637351
1903.555196	330.318722	62.642356
1902.942254	292.247729	62.647361
1902.225584	257.643793	62.652366
1901.519727	221.658347	62.657370
1900.490259	192.406899	62.662375
1899.931760	160.588297	62.667380
1899.191477	133.045465	62.672385
1898.417133	102.759401	62.677390
1897.692140	79.554119	62.682394
1896.955519	54.601845	62.687399
1896.083778	25.709691	62.692404
1895.434099	6.491794	62.697409
1894.728395	-5.931452	62.702414
1893.888991	-10.700893	62.707418
1892.376042	-10.175143	62.712423
1890.609030	14.837260	62.717428
1889.515971	33.325965	62.722433
1888.790100	43.381038	62.727438
1888.650039	40.487546	62.732442
1888.547878	45.144935	62.737447
1888.324806	44.951800	62.742452
1888.327214	34.860420	62.747457
1887.199253	38.160463	62.752462
1886.352032	30.932159	62.757466
1885.320187	50.429897	62.762471
1884.802367	48.279214	62.767476
1884.563733	43.562610	62.772481
1883.390828	49.408734	62.777486
1883.387590	54.744294	62.782490
1882.683954	61.141979	62.787495
1882.072977	60.840118	62.792500
1881.059663	59.802606	62.797505
1880.049142	64.539568	62.802510
1880.137668	56.404154	62.807514
1879.607898	66.141099	62.812519
1878.850731	58.095801	62.817524
1878.193934	54.778138	62.822529
1877.204174	62.446571	62.827534
1876.435371	58.307736	62.832538
1875.427016	64.809000	62.837543
1874.950246	66.731458	62.842548
1874.980957	66.229942	62.847553
1874.163334	64.240403	62.852558
1873.578426	66.348768	62.857562
1872.779471	74.814831	62.862567
1871.755242	68.551348	62.867572
1871.750381	67.599731	62.872577
1871.196236	70.587902	62.877582
1871.046481	61.794869	62.882586
1869.620514	70.190169	62.887591
1868.324164	60.243483	62.892596
1868.186852	78.202022	62.897601
1867.455945	77.307335	62.902606
1867.182453	59.860531	62.907610
1866.453516	73.480100	62.912615
1865.838903	71.295899	62.917620
1865.130596	62.413353	62.922625
1864.125243	72.604291	62.927630
1863.244954	70.711438	62.932634
1862.471118	69.312627	62.937639
1862.444615	71.795966	62.942644
1862.513071	66.571695	62.947649
1860.749531	70.628698	62.952654
1860.417959	68.746495	62.957658
1860.096035	67.238082	62.962663
1859.177504	72.105530	62.967668
1858.763020	62.810471	62.972673
1857.566003	74.274508	62.977678
1857.211415	67.300722	62.982682
1856.568532	71.782197	62.987687
1856.111359	68.465957	62.992692
1855.390806	66.967223	62.997697
1854.340131	81.596693	63.002702
1853.963275	75.895913	63.007706
1853.182120	76.294452	63.012711
1852.259299	76.485246	63.017716
1851.804426	70.954555	63.022721
1850.907102	78.745523	63.027726
1850.411260	74.711587	63.032730
1849.577036	73.101590	63.037735
1848.906931	81.406850	63.042740
1848.596066	72.549507	63.047745
1847.498366	82.930166	63.052750
1847.648189	75.578234	63.057754
1846.910030	79.584399	63.062759
1845.768335	78.573592	63.067764
1845.329207	68.579112	63.072769
1844.311492	77.097264	63.077774
1844.704867	75.453196	63.082778
1843.432525	72.564445	63.087783
1842.057794	82.432418	63.092788
1842.469958	70.422996	63.097793
1841.375821	76.725004	63.102798
1840.538843	74.371111	63.107802
1840.137275	77.439142	63.112807
1839.785912	78.135300	63.117812
1838.711276	76.779528	63.122817
1837.533197	79.160290	63.127822
1837.722736	68.447808	63.132826
1836.989321	73.460914	63.137831
1836.300083	85.238583	63.142836
1835.279682	64.198159	63.147841
1834.449627	75.764788	63.152846
1834.338350	79.925308	63.157850
1833.389469	69.824112	63.162855
1832.498117	75.609788	63.167860
1832.581238	70.627621	63.172865
1831.767823	80.734478	63.177870
1831.074597	70.488606	63.182874
1830.459315	80.787934	63.187879
1829.797330	78.172862	63.192884
1829.354378	70.922946	63.197889
1828.410037	77.723154	63.202894
1827.939862	74.883657	63.207898
1827.405414	71.387301	63.212903
1825.716283	77.629251	63.217908
1825.555794	70.186247	63.222913
1824.928504	80.605756	63.227918
1824.208711	72.570306	63.232922
1823.644228	76.509472	63.237927
1822.781936	71.451922	63.242932
1822.421589	70.212972	63.247937
1821.534645	76.915757	63.252942
1821.162347	80.050108	63.257946
1820.451675	83.826406	63.262951
1819.211210	74.801287	63.267956
1818.688419	69.926376	63.272961
1818.667853	75.289922	63.277966
1818.094600	76.939124	63.282970
1817.259244	80.449787	63.287975
1816.241754	72.690276	63.292980
1816.025013	75.563377	63.297985
1815.242339	81.694509	63.302990
1814.570832	74.879866	63.307994
1814.100983	74.736963	63.312999
1813.270858	82.845286	63.318004
1812.719810	77.107518	63.323009
1811.212482	76.020745	63.328014
1811.060217	77.997342	63.333018
1810.453670	72.692600	63.338023
1809.855641	74.465588	63.343028
1808.959450	70.943101	63.348033
1808.054735	87.213128	63.353038
1808.429703	75.222224	63.358042
1807.422346	72.184178	63.363047
1806.591622	76.263399	63.368052
1805.879192	70.324178	63.373057
1805.404142	86.844525	63.378062
1804.695376	79.110109	63.383066
1804.135074	77.453474	63.388071
1803.535878	81.033874	63.393076
1802.442367	81.213944	63.398081
1801.599591	78.621281	63.403086
1801.113911	78.178114	63.408090
1800.693288	85.308337	63.413095
1799.768899	84.013878	63.418100
1799.297336	80.920711	63.423105
1798.491550	85.371299	63.428110
1797.913714	83.471439	63.433114
1797.343800	90.798841	63.438119
1796.417860	88.765023	63.443124
1796.269824	78.738515	63.448129
1795.432991	88.423318	63.453134
1794.827575	84.003085	63.458138
1794.543152	86.456419	63.463143
1793.641356	80.332800	63.468148
1792.945730	73.380067	63.473153
1791.965199	79.807558	63.478158
1791.315784	82.137502	63.483162
1790.778885	83.809322	63.488167
1790.008088	92.130588	63.493172
1789.606426	81.817921	63.498177
1789.015004	90.568026	63.503182
1788.442328	76.537180	63.508186
1787.796714	79.375886	63.513191
1786.286818	83.198689	63.518196
1785.782104	82.955671	63.523201
1785.078045	80.098129	63.528206
1784.563352	83.119477	63.533210
1784.372538	82.364552	63.538215
1783.309141	83.959133	63.543220
1782.839257	74.658693	63.548225
1782.335579	75.361701	63.553230
1781.626825	84.012162	63.558234
1781.483368	80.180904	63.563239
1780.735312	81.589787	63.568244
1779.825606	80.091150	63.573249
1778.642156	88.214593	63.578254
1778.147227	78.180100	63.583258
1777.492018	90.632057	63.588263
1776.665419	86.849363	63.593268
1776.532054	83.965847	63.598273
1775.785282	91.581542	63.603278
1775.148026	84.340413	63.608282
1774.497250	81.980624	63.613287
1773.169445	86.034719	63.618292
1772.459678	82.555178	63.623297
1771.854806	84.322954	63.628302
1771.956306	78.284441	63.633306
1770.995795	79.563060	63.638311
1770.291156	83.936090	63.643316
1769.962355	73.801100	63.648321
1769.446150	76.073622	63.653326
1768.834641	77.304700	63.658330
1767.545484	76.563358	63.663335
1766.482315	81.745548	63.668340
1766.129187	82.265374	63.673345
1765.493423	80.944014	63.678350
1764.901581	76.745568	63.683354
1764.733858	83.490269	63.688359
1763.753678	82.185760	63.693364
1763.757775	76.407150	63.698369
1762.853070	84.972039	63.703374
1761.618653	80.645404	63.708378
1760.769900	77.484414	63.713383
1759.834012	77.770358	63.718388
1759.420010	79.419512	63.723393
1759.276553	82.489139	63.728398
1758.568664	88.125853	63.733402
1758.157847	74.966618	63.738407
1757.312846	91.119940	63.743412
1757.200821	80.898479	63.748417
1756.028210	89.106944	63.753422
1754.888033	83.767113	63.758426
1754.511297	83.898021	63.763431
1753.440233	87.455601	63.768436
1753.119854	83.969418	63.773441
1752.671068	92.162277	63.778446
1752.361286	86.353088	63.783450
1751.547746	86.096045	63.788455
1750.092943	88.782574	63.793460
1749.654040	77.646341	63.798465
1749.161948	80.317168	63.803470
1748.581467	85.846914	63.808474
1748.046166	79.095815	63.813479
1747.472447	89.989389	63.818484
1747.080753	84.729386	63.823489
1745.838527	90.566088	63.828494
1745.081161	82.019379	63.833498
1744.611919	83.172673	63.838503
1743.826320	87.454487	63.843508
1743.448338	76.412662	63.848513
1742.886271	81.537351	63.853518
1742.433131	80.147567	63.858522
1741.636327	76.461083	63.863527
1740.509650	80.171005	63.868532
1739.972896	75.044435	63.873537
1739.187225	80.098981	63.878542
1738.739377	86.310998	63.883546
1738.291806	77.751360	63.888551
1737.548118	89.107178	63.893556
1736.751616	84.379835	63.898561
1735.703154	91.961452	63.903566
1735.024405	87.322642	63.908570
1734.698443	82.995239	63.913575
1733.908617	85.027369	63.918580
1733.784399	79.579806	63.923585
1732.759022	80.922359	63.928590
1732.617961	79.153420	63.933594
1731.719437	78.023616	63.938599
1730.535268	85.336620	63.943604
1730.099914	82.644578	63.948609
1729.731822	85.379295	63.953614
1728.882832	84.735220	63.958618
1728.652889	78.478110	63.963623
1727.057970	91.621810	63.968628
1726.250499	79.889673	63.973633
1725.545324	87.276415	63.978638
1724.953707	88.603694	63.983642
1725.015492	86.529719	63.988647
1724.182929	89.119008	63.993652
1724.077089	82.048962	63.998657
1723.887026	80.902831	64.003662
1722.631423	81.725280	64.008666
1721.636467	83.274321	64.013671
1720.831804	88.551092	64.018676
1720.418177	81.063147	64.023681
1719.706553	84.536839	64.028686
1718.403679	89.020671	64.033690
1717.736192	82.418311	64.038695
1717.033921	87.964253	64.043700
1716.561351	83.690102	64.048705
1716.302599	89.914666	64.053710
1715.412865	85.604270	64.058714
1715.132763	75.508867	64.063719
1714.448611	81.700069	64.068724
1714.495720	83.758546	64.073729
1713.261693	88.830699	64.078734
1712.484334	75.895280	64.083738
1712.077291	81.556757	64.088743
1711.363164	87.636027	64.093748
1710.143254	80.094799	64.098753
1709.281719	84.905932	64.103758
1708.352783	88.893549	64.108762
1708.144719	77.616581	64.113767
1707.752167	88.170716	64.118772
1707.284633	86.295936	64.123777
1706.772698	93.046428	64.128782
1705.871491	85.618583	64.133786
1704.920914	81.872956	64.138791
1704.072383	87.618754	64.143796
1703.720022	79.722105	64.148801
1702.944803	83.589110	64.153806
1702.433978	86.184071	64.158810
1702.424417	75.518986	64.163815
1701.292883	91.421355	64.168820
1700.657424	84.455937	64.173825
1699.756070	83.548948	64.178830
1698.945447	90.551892	64.183834
1698.865731	79.492662	64.188839
1697.959301	84.422896	64.193844
1697.194541	83.719720	64.198849
1696.259965	85.765391	64.203854
1695.782132	85.825632	64.208858
1695.029760	80.720705	64.213863
1694.574053	90.313452	64.218868
1694.248351	79.493573	64.223873
1693.034260	78.330328	64.228878
1692.592337	87.010964	64.233882
1692.160892	86.682208	64.238887
1691.260998	93.002307	64.243892
1691.467794	85.187154	64.248897
1690.466576	90.935133	64.253902
1689.884024	86.232170	64.258906
1688.395939	87.260302	64.263911
1687.031203	84.837324	64.268916
1686.337953	83.179756	64.273921
1686.567188	94.384194	64.278926
1685.784287	72.598060	64.283930
1684.780898	86.062559	64.288935
1684.324391	77.575320	64.293940
1684.085144	84.279341	64.298945
1683.363677	82.973193	64.303950
1682.880444	76.308462	64.308954
1682.685447	70.868996	64.313959
1681.427824	85.903553	64.318964
1680.475225	72.989680	64.323969
1680.056674	79.379976	64.328974
1679.151376	84.021448	64.333978
1679.254767	78.766397	64.338983
1677.766798	86.648084	64.343988
1677.176109	86.866607	64.348993
1676.325357	83.124057	64.353998
1675.731507	85.647055	64.359002
1675.564832	75.363328	64.364007
1675.036711	88.716066	64.369012
1674.294147	79.522047	64.374017
1673.019258	87.764135	64.379022
1672.576506	79.080744	64.384026
1671.965994	75.681665	64.389031
1671.369562	85.886557	64.394036
1671.169124	86.842619	64.399041
1670.657891	83.989174	64.404046
1669.656069	86.504439	64.409050
1668.840791	75.866421	64.414055
1667.859012	86.708125	64.419060
1667.349379	78.328679	64.424065
1666.966939	85.580583	64.429070
1665.533783	89.823356	64.434074
1665.072395	81.964534	64.439079
1664.732894	84.671061	64.444084
1664.245622	81.104169	64.449089
1663.700315	88.123322	64.454094
1663.139780	80.791194	64.459098
1662.960437	87.230230	64.464103
1661.512585	86.354874	64.469108
1660.911289	77.171538	64.474113
1660.574585	82.517489	64.479118
1659.154391	83.435501	64.484122
1658.386916	81.546878	64.489127
1657.885756	84.083540	64.494132
1657.186439	83.723224	64.499137
1656.735313	81.565146	64.504142
1656.123268	82.462014	64.509146
1655.793467	75.493791	64.514151
1655.398927	85.530991	64.519156
1654.922083	83.676625	64.524161
1653.628817	76.986038	64.529166
1652.404234	81.637236	64.534170
1652.132492	77.152999	64.539175
1651.628377	91.686241	64.544180
1651.446663	79.906770	64.549185
1650.643164	80.893979	64.554190
1649.487525	81.539730	64.559194
1649.114010	75.340136	64.564199
1648.377066	87.771973	64.569204
1647.976782	82.218460	64.574209
1646.974405	73.964610	64.579214
1645.952624	83.894869	64.584218
1645.774159	79.055187	64.589223
1645.130942	87.961774	64.594228
1644.449130	82.377290	64.599233
1643.458502	85.048484	64.604238
1642.166445	87.911071	64.609242
1642.086347	74.987920	64.614247
1641.881203	75.028505	64.619252
1641.289410	79.016198	64.624257
1640.886498	81.217127	64.629262
1640.001550	82.838610	64.634266
1639.201721	82.104753	64.639271
1638.196096	91.338580	64.644276
1637.974435	80.864892	64.649281
1637.313177	80.362915	64.654286
1636.309075	84.815088	64.659290
1635.653299	71.652230	64.664295
1634.839663	87.508841	64.669300
1633.832467	78.590273	64.674305
1633.907985	82.467224	64.679310
1633.611621	87.278481	64.684314
1633.147144	81.140648	64.689319
1631.728698	89.175320	64.694324
1630.886137	74.055137	64.699329
1630.634507	83.438841	64.704334
1629.747128	90.088135	64.709338
1629.684778	75.854847	64.714343
1628.319067	78.249737	64.719348
1627.626161	70.889768	64.724353
1627.154511	75.648443	64.729358
1626.578624	83.689609	64.734362
1626.369852	72.423814	64.739367
1625.298267	84.449914	64.744372
1624.379732	85.972658	64.749377
1623.693734	85.635467	64.754382
1623.203119	83.603519	64.759386
1622.810056	79.064442	64.764391
1622.098744	84.667034	64.769396
1620.861056	80.894513	64.774401
1620.567337	76.751247	64.779406
1619.631821	89.083748	64.784410
1619.724786	72.748903	64.789415
1618.923604	79.849711	64.794420
1618.018834	86.766702	64.799425
1617.071868	86.540360	64.804430
1616.132678	92.623869	64.809434
1616.186058	85.132716	64.814439
1615.667465	86.246563	64.819444
1614.826824	82.705861	64.824449
1613.825481	80.097455	64.829454
1613.036102	87.445556	64.834458
1612.723609	76.230932	64.839463
1611.882479	94.656093	64.844468
1611.841534	82.299166	64.849473
1610.813441	85.958784	64.854478
1609.475740	86.717058	64.859482
1609.775018	76.405046	64.864487
1608.900740	86.468004	64.869492
1608.404743	82.692772	64.874497
1607.567080	81.561228	64.879502
1606.524532	81.603970	64.884506
1606.140369	74.250150	64.889511
1605.608513	79.926735	64.894516
1605.010867	78.667171	64.899521
1604.132963	75.564487	64.904526
1603.098538	83.288994	64.909530
1602.596177	76.715634	64.914535
1601.992092	74.632333	64.919540
1601.825054	76.256463	64.924545
1601.077887	83.966871	64.929550
1599.640772	84.605325	64.934554
1599.243492	75.332825	64.939559
1598.582802	76.735761	64.944564
1598.204079	84.865457	64.949569
1598.013448	79.846360	64.954574
1596.719815	83.221736	64.959578
1596.502626	67.943870	64.964583
1595.348224	74.235037	64.969588
1594.922574	73.050653	64.974593
1594.294208	71.020098	64.979598
1593.141019	70.512712	64.984602
1592.637285	66.073232	64.989607
1591.972769	80.800686	64.994612
1591.239492	78.141815	64.999617
1591.237389	78.019255	65.004622
1590.875952	84.924045	65.009626
1589.811841	82.909105	65.014631
1588.873382	85.039009	65.019636
1588.014048	83.874644	65.024641
1587.997660	74.223080	65.029646
1586.518397	84.681791	65.034650
1585.991750	78.211643	65.039655
1585.313510	83.231812	65.044660
1584.788169	82.894337	65.049665
1584.643105	82.425478	65.054670
1583.745629	85.477715	65.059674
1583.228192	71.925462	65.064679
1582.165401	77.971841	65.069684
1581.652521	77.473112	65.074689
1581.101759	84.502602	65.079694
1580.749322	78.433715	65.084698
1580.021010	72.080771	65.089703
1578.743385	77.006936	65.094708
1578.275191	82.383247	65.099713
1577.967673	71.227770	65.104718
1577.143873	84.274245	65.109722
1576.691974	74.942620	65.114727
1575.733891	72.026155	65.119732
1574.976927	65.486953	65.124737
1574.663483	65.191508	65.129742
1573.930226	80.093891	65.134746
1573.040986	72.637400	65.139751
1572.527285	74.056411	65.144756
1571.669936	78.761259	65.149761
1570.858485	74.395906	65.154766
1569.899093	87.236844	65.159770
1569.402243	75.608392	65.164775
1568.910157	76.088821	65.169780
1568.337179	67.607510	65.174785
1568.180382	65.617154	65.179790
1567.524986	81.033878	65.184794
1566.910307	67.175382	65.189799
1565.809036	73.737244	65.194804
1565.345614	76.310502	65.199809
1564.818646	71.691789	65.204814
1563.079629	81.510526	65.209818
1562.794652	74.901059	65.214823
1562.225575	67.403166	65.219828
1561.746192	79.839817	65.224833
1561.346983	73.027725	65.229838
1560.972861	74.957580	65.234842
1560.260330	72.273345	65.239847
1559.390025	76.149185	65.244852
1558.477399	68.735843	65.249857
1558.243321	68.542908	65.254862
1556.907606	80.749768	65.259866
1555.942580	71.102286	65.264871
1555.532390	79.706921	65.269876
1555.243413	73.571187	65.274881
1554.972558	66.156799	65.279886
1554.402696	77.970726	65.284890
1553.811077	68.527269	65.289895
1552.720494	74.007206	65.294900
1552.097970	77.742751	65.299905
1551.574157	75.899024	65.304910
1550.198582	75.046941	65.309914
1549.676204	76.024204	65.314919
1549.366288	72.962179	65.319924
1549.008646	63.057341	65.324929
1548.429266	74.369722	65.329934
1547.010738	78.187596	65.334938
1546.115126	70.046144	65.339943
1545.596764	81.167482	65.344948
1544.928880	82.003861	65.349953
1544.992255	77.406466	65.354958
1544.476437	80.316066	65.359962
1543.407531	82.974502	65.364967
1542.457454	78.238518	65.369972
1541.918543	80.003746	65.374977
1541.820956	73.730367	65.379982
1541.161184	76.637610	65.384986
1539.779759	71.713124	65.389991
1539.014128	69.871556	65.394996
1538.393286	75.511826	65.400001
1538.261481	75.592806	65.405006
1537.545733	84.187651	65.410010
1536.986157	76.158385	65.415015
1536.063558	77.841079	65.420020
1535.323859	77.247512	65.425025
1535.039939	70.991128	65.430030
1534.085900	81.068351	65.435034
1533.061872	71.934888	65.440039
1532.732907	78.470236	65.445044
1532.159211	82.516577	65.450049
1531.821239	78.397703	65.455054
1531.093061	81.569713	65.460058
1530.231260	78.437689	65.465063
1529.279200	80.579236	65.470068
1528.614064	78.614466	65.475073
1528.593924	77.154340	65.480078
1527.807412	85.853474	65.485082
1526.798409	67.110667	65.490087
1526.125138	76.242817	65.495092
1525.439386	81.855559	65.500097
1525.274065	79.144303	65.505102
1523.891325	82.677378	65.510106
1523.426536	70.078739	65.515111
1523.039961	70.461983	65.520116
1522.577222	74.702006	65.525121
1521.950572	67.438782	65.530126
1520.901629	80.610928	65.535130
1520.332624	77.621617	65.540135
1519.736318	75.496099	65.545140
1518.770100	73.645411	65.550145
1517.945686	68.816931	65.555150
1517.153194	69.217371	65.560154
1516.951492	76.778033	65.565159
1516.628795	76.987122	65.570164
1516.091402	71.614705	65.575169
1515.120613	76.105778	65.580174
1513.978496	78.484117	65.585178
1513.744442	68.397216	65.590183
1513.488961	63.356901	65.595188
1512.352163	79.506152	65.600193
1511.402003	72.094062	65.605198
1510.840683	83.066110	65.610202
1510.447599	69.684937	65.615207
1509.704544	74.377946	65.620212
1509.356961	74.933194	65.625217
1508.087278	63.173693	65.630222
1507.389431	72.912155	65.635226
1506.866797	73.892621	65.640231
1506.689018	75.136835	65.645236
1505.881541	75.282612	65.650241
1504.761400	73.137841	65.655246
1504.047738	79.447315	65.660250
1503.847804	73.141319	65.665255
1503.487280	77.749884	65.670260
1502.379931	76.812624	65.675265
1501.867955	73.509898	65.680270
1500.622462	83.146161	65.685274
1500.178784	77.307838	65.690279
1499.661137	80.118386	65.695284
1499.013658	80.893186	65.700289
1499.014157	80.568359	65.705294
1497.827762	72.971463	65.710298
1497.110489	69.852755	65.715303
1496.492574	76.317328	65.720308
1495.789013	79.846562	65.725313
1495.559653	80.761500	65.730318
1494.218331	85.524360	65.735322
1493.479825	87.813336	65.740327
1493.266177	78.011776	65.745332
1492.728082	80.067048	65.750337
1492.494814	73.827853	65.755342
1491.058054	79.944735	65.760346
1490.462521	69.358610	65.765351
1490.170005	74.394768	65.770356
1489.074683	79.066493	65.775361
1488.381962	67.470779	65.780366
1487.419421	79.063263	65.785370
1486.973338	68.831864	65.790375
1486.329012	71.769779	65.795380
1485.930199	75.895568	65.800385
1485.765719	78.834499	65.805390
1484.328262	77.386726	65.810394
1483.949420	73.690680	65.815399
1483.714976	70.499974	65.820404
1482.729929	78.237169	65.825409
1481.964432	72.919936	65.830414
1481.123084	81.613600	65.835418
1480.266588	73.394994	65.840423
1480.050469	74.844001	65.845428
1479.635437	76.781945	65.850433
1478.857419	69.281011	65.855438
1477.945980	74.559038	65.860442
1477.573794	62.672690	65.865447
1477.066554	70.395449	65.870452
1475.994508	79.822801	65.875457
1475.207849	71.115275	65.880462
1474.369774	78.024856	65.885466
1474.123254	73.844150	65.890471
1473.792517	72.054913	65.895476
1472.715215	78.892126	65.900481
1471.639796	74.168210	65.905486
1471.068697	75.895988	65.910490
1470.666811	71.038220	65.915495
1470.830777	63.486934	65.920500
1469.522776	81.032223	65.925505
1468.869076	69.013992	65.930510
1467.852964	73.518591	65.935514
1467.463405	71.800206	65.940519
1466.950266	69.828644	65.945524
1465.818915	72.052325	65.950529
1465.297285	72.365577	65.955534
1464.609305	78.680440	65.960538
1464.475886	70.722244	65.965543
1463.808363	65.980815	65.970548
1462.386135	71.694846	65.975553
1462.013939	66.737744	65.980558
1461.573505	69.871922	65.985562
1461.384581	66.908955	65.990567
1460.348393	69.522796	65.995572
1459.507404	74.748630	66.000577
1459.119267	69.664749	66.005582
1458.174426	72.798669	66.010586
1457.345483	69.759224	66.015591
1456.660924	77.179005	66.020596
1455.690116	84.177499	66.025601
1455.670419	73.343743	66.030606
1455.187416	74.983405	66.035610
1454.254099	78.135996	66.040615
1453.669332	73.895510	66.045620
1453.163565	78.270117	66.050625
1452.482814	72.475794	66.055630
1451.278710	69.256277	66.060634
1450.508922	63.846699	66.065639
1449.964714	63.575331	66.070644
1449.435680	81.424181	66.075649
1449.311068	71.354589	66.080654
1448.794674	76.905734	66.085658
1447.817262	75.930499	66.090663
1446.972953	72.597027	66.095668
1446.484045	72.017245	66.100673
1445.954185	67.468410	66.105678
1444.597427	79.511497	66.110682
1444.138708	74.307946	66.115687
1443.496416	75.080358	66.120692
1443.239901	77.406281	66.125697
1442.680319	64.348068	66.130702
1441.446530	76.961399	66.135706
1441.024883	63.559561	66.140711
1440.738417	71.414394	66.145716
1439.377800	68.203990	66.150721
1438.770940	60.787838	66.155726
1437.837523	76.710812	66.160730
1437.372323	68.904704	66.165735
1436.885513	63.950055	66.170740
1436.556075	70.288358	66.175745
1436.207933	62.619770	66.180750
1435.208105	78.300985	66.185754
1434.455383	70.209411	66.190759
1434.044399	71.821860	66.195764
1433.327729	70.146011	66.200769
1432.417819	67.319721	66.205774
1431.312988	62.783431	66.210778
1430.799545	67.075678	66.215783
1430.673517	70.388549	66.220788
1430.051449	75.483399	66.225793
1428.719413	65.865930	66.230798
1427.867490	72.374015	66.235802
1427.876128	62.207559	66.240807
1427.169920	62.786703	66.245812
1426.964916	64.953047	66.250817
1426.607377	51.630923	66.255822
1425.302456	65.742644	66.260826
1424.629641	67.432981	66.265831
1424.070260	64.147273	66.270836
1422.917304	74.713460	66.275841
1422.452196	66.219781	66.280846
1422.189302	72.041299	66.285850
1421.633860	69.652265	66.290855
1420.204471	68.173285	66.295860
1419.409527	70.622638	66.300865
1419.243426	69.281911	66.305870
1418.818750	68.043787	66.310874
1418.332815	66.842208	66.315879
1417.259479	64.568611	66.320884
1416.086243	79.170357	66.325889
1415.908582	77.292140	66.330894
1415.287999	74.631182	66.335898
1414.610748	69.415066	66.340903
1413.856660	68.539967	66.345908
1413.020724	75.244215	66.350913
1412.676426	63.708272	66.355918
1411.817118	74.700880	66.360922
1411.510896	73.349309	66.365927
1410.782218	71.981309	66.370932
1409.738521	73.454632	66.375937
1409.579504	63.888845	66.380942
1408.981504	65.658759	66.385946
1407.889059	65.670088	66.390951
1406.914822	70.273708	66.395956
1406.160422	73.670692	66.400961
1406.103575	60.609857	66.405966
1405.624794	71.672867	66.410970
1405.052701	65.347196	66.415975
1404.031245	67.430429	66.420980
1403.605841	65.495399	66.425985
1403.075635	54.244487	66.430990
1401.877299	69.693899	66.435994
1401.110970	71.903739	66.440999
1400.671787	62.842967	66.446004
1400.074107	69.786891	66.451009
1399.848084	70.239251	66.456014
1398.829775	68.855792	66.461018
1397.809526	72.913211	66.466023
1397.581775	71.629594	66.471028
1397.000857	67.516249	66.476033
1396.530134	61.434670	66.481038
1395.317392	72.024561	66.486042
1394.419182	64.916511	66.491047
1394.558649	66.960291	66.496052
1393.397082	70.390461	66.501057
1392.517026	68.791059	66.506062
1391.758347	65.089178	66.511066
1391.363675	66.454608	66.516071
1391.164097	65.458255	66.521076
1390.376666	75.447524	66.526081
1389.568147	64.475819	66.531086
1388.792768	68.048031	66.536090
1387.917353	72.533446	66.541095
1387.642767	60.059168	66.546100
1386.958181	72.381782	66.551105
1386.299083	79.710796	66.556110
1385.360154	77.109912	66.561114
1385.074069	72.102865	66.566119
1384.812229	70.206494	66.571124
1383.193956	71.597696	66.576129
1382.670232	63.715752	66.581134
1382.185191	65.082932	66.586138
1381.466364	65.205195	66.591143
1381.188875	56.524011	66.596148
1380.462152	66.749634	66.601153
1379.698533	68.763504	66.606158
1379.359237	64.092931	66.611162
1378.007933	61.981812	66.616167
1376.864854	66.240114	66.621172
1376.459238	76.156076	66.626177
1376.272986	66.206687	66.631182
1375.749491	61.128574	66.636186
1375.383003	61.566995	66.641191
1374.933510	57.043254	66.646196
1373.644246	76.160987	66.651201
1373.461357	66.100675	66.656206
1372.749899	65.707675	66.661210
1371.379381	66.037618	66.666215
1370.630212	74.866463	66.671220
1369.829180	80.735685	66.676225
1369.747610	63.454062	66.681230
1369.079467	75.892340	66.686234
1368.634710	77.297275	66.691239
1368.130780	63.782382	66.696244
1367.390599	75.202347	66.701249
1366.818739	61.911147	66.706254
1365.404267	62.322198	66.711258
1364.658755	63.790714	66.716263
1364.594111	66.308492	66.721268
1363.833822	67.763588	66.726273
1362.778196	72.271350	66.731278
1362.297186	74.481576	66.736282
1361.591399	71.804215	66.741287
1361.593710	63.755074	66.746292
1360.590954	75.948498	66.751297
1359.948221	61.154671	66.756302
1358.927348	73.428246	66.761306
1358.259868	67.510418	66.766311
1357.954059	62.596402	66.771316
1357.180633	73.428709	66.776321
1356.387820	70.071316	66.781326
1355.863604	69.933986	66.786330
1354.961468	70.399215	66.791335
1355.015250	63.411082	66.796340
1353.883766	78.389413	66.801345
1353.064598	66.444843	66.806350
1352.517525	60.499994	66.811354
1352.006903	66.550132	66.816359
1351.476926	65.205756	66.821364
1350.214863	70.815530	66.826369
1349.861538	63.234518	66.831374
1349.400285	69.185345	66.836378
1348.628180	72.484231	66.841383
1347.877974	68.128149	66.846388
1346.907082	68.908668	66.851393
1346.475472	71.036925	66.856398
1346.174207	57.409401	66.861402
1345.303964	63.792681	66.866407
1344.281577	62.337352	66.871412
1343.417489	68.748042	66.876417
1343.317401	63.369231	66.881422
1342.701329	66.181258	66.886426
1342.610298	70.108317	66.891431
1341.553896	67.940873	66.896436
1340.580193	64.333119	66.901441
1340.297106	63.637056	66.906446
1339.154373	64.717714	66.911450
1338.014953	70.129797	66.916455
1337.983726	61.863637	66.921460
1337.312663	73.349888	66.926465
1336.984808	56.478024	66.931470
1336.326905	61.723666	66.936474
1334.974607	59.874507	66.941479
1334.692819	65.317401	66.946484
1333.788523	72.994491	66.951489
1333.632347	65.483064	66.956494
1333.075572	71.863824	66.961498
1331.725550	70.347046	66.966503
1331.610080	59.038102	66.971508
1330.656572	72.854294	66.976513
1330.408831	58.461315	66.981518
1329.248660	67.417008	66.986522
1328.500329	60.997953	66.991527
1328.337279	55.819971	66.996532
1327.620843	64.556880	67.001537
1326.863959	63.021500	67.006542
1326.034785	66.476123	67.011546
1325.325302	64.073756	67.016551
1325.224427	58.661958	67.021556
1323.906525	73.933285	67.026561
1322.891526	61.518389	67.031566
1322.176034	65.754465	67.036570
1321.846549	62.608854	67.041575
1321.482818	70.903334	67.046580
1321.413892	69.359505	67.051585
1320.816062	62.101229	67.056590
1319.507009	61.536745	67.061594
1318.905911	75.419917	67.066599
1318.439280	59.180409	67.071604
1317.319562	72.948912	67.076609
1316.849245	56.079204	67.081614
1316.252101	66.478204	67.086618
1315.935092	60.627677	67.091623
1315.062734	59.918071	67.096628
1313.741851	70.515721	67.101633
1313.337069	67.615474	67.106638
1312.893787	60.827800	67.111642
1312.531746	76.551142	67.116647
1311.495036	64.177549	67.121652
1310.416018	77.963242	67.126657
1310.025767	65.505791	67.131662
1309.808882	65.396880	67.136666
1309.402292	64.630569	67.141671
1308.574241	60.316842	67.146676
1307.456665	67.225166	67.151681
1306.950826	65.028550	67.156686
1306.644978	69.054418	67.161690
1305.435706	68.701161	67.166695
1305.050374	60.011905	67.171700
1304.307616	70.855114	67.176705
1303.932603	65.201469	67.181710
1302.723978	70.124668	67.186714
1301.525699	67.476744	67.191719
1301.579803	64.328496	67.196724
1300.872908	68.768217	67.201729
1299.990025	66.103264	67.206734
1300.142066	63.887206	67.211738
1299.541845	67.854221	67.216743
1298.714061	64.467716	67.221748
1297.350028	74.723725	67.226753
1297.386338	64.937663	67.231758
1296.565455	67.290249	67.236762
1295.415108	72.978480	67.241767
1295.044571	67.421897	67.246772
1294.585787	74.255445	67.251777
1293.828278	65.846140	67.256782
1292.592982	66.517330	67.261786
1291.881756	73.854646	67.266791
1291.919576	60.532770	67.271796
1291.239172	67.213892	67.276801
1290.774176	58.592502	67.281806
1289.965376	60.738160	67.286810
1289.080833	63.802622	67.291815
1288.631685	63.530367	67.296820
1288.156745	67.499542	67.301825
1287.176803	71.414971	67.306830
1286.340954	60.450814	67.311834
1285.639888	69.861812	67.316839
1285.784035	62.163869	67.321844
1284.275329	65.362268	67.326849
1283.268983	67.643420	67.331854
1282.728368	64.146604	67.336858
1282.472821	72.288265	67.341863
1282.449831	71.472004	67.346868
1281.548787	67.882684	67.351873
1281.010610	66.922832	67.356878
1279.848319	66.014907	67.361882
1278.975838	73.917191	67.366887
1278.390268	66.396775	67.371892
1277.721074	74.232043	67.376897
1277.302716	66.554152	67.381902
1277.051858	65.739430	67.386906
1275.871006	78.074738	67.391911
1275.189114	69.085704	67.396916
1274.352885	71.869674	67.401921
1274.333265	70.925142	67.406926
1273.562840	74.165434	67.411930
1272.394384	69.006968	67.416935
1272.131826	60.429087	67.421940
1271.376862	75.718158	67.426945
1270.732369	75.413888	67.431950
1270.026811	69.352331	67.436954
1269.217079	69.356613	67.441959
1268.672671	66.090641	67.446964
1268.360899	66.777424	67.451969
1267.139402	70.515223	67.456974
1266.659418	70.416611	67.461978
1265.775314	73.659211	67.466983
1265.578510	74.329290	67.471988
1264.547949	79.290427	67.476993
1263.709171	72.346447	67.481998
1263.250464	71.750859	67.487002
1262.396521	70.380744	67.492007
1262.458470	72.741197	67.497012
1261.567661	72.498173	67.502017
1260.781376	73.749271	67.507022
1259.927560	61.633636	67.512026
1259.461903	72.833343	67.517031
1259.367494	65.785198	67.522036
1257.787813	76.807231	67.527041
1257.241393	66.705397	67.532046
1256.918011	68.847997	67.537050
1256.429396	71.929939	67.542055
1255.363103	69.554367	67.547060
1254.217762	66.298798	67.552065
1253.813006	68.596266	67.557070
1253.611433	65.942842	67.562074
1253.407419	63.255114	67.567079
1252.335245	63.607067	67.572084
1251.335865	63.141612	67.577089
1250.710037	61.440334	67.582094
1250.382484	64.327929	67.587098
1249.153916	69.686412	67.592103
1248.665078	60.706119	67.597108
1248.004951	61.233829	67.602113
1247.228903	58.285400	67.607118
1247.480500	61.249636	67.612122
1246.115968	65.546359	67.617127
1245.403132	61.370455	67.622132
1244.500603	65.987956	67.627137
1244.058228	66.864245	67.632142
1243.864906	61.681623	67.637146
1243.142901	70.794757	67.642151
1242.125741	64.405864	67.647156
1241.716978	77.179810	67.652161
1241.078741	74.442857	67.657166
1240.433685	73.955755	67.662170
1239.113227	71.279980	67.667175
1238.885506	64.120572	67.672180
1238.095748	67.717188	67.677185
1238.036604	76.291250	67.682190
1236.929375	70.230499	67.687194
1236.144302	77.316216	67.692199
1236.049146	66.450337	67.697204
1235.548518	66.697217	67.702209
1234.033537	65.291881	67.707214
1233.790833	65.921951	67.712218
1232.974492	73.768010	67.717223
1232.532414	67.409098	67.722228
1231.271006	71.143798	67.727233
1230.830927	66.736863	67.732238
1230.679707	63.711155	67.737242
1229.678765	70.820160	67.742247
1229.279839	65.012636	67.747252
1228.100457	68.880951	67.752257
1227.507314	71.293537	67.757262
1227.409800	65.874904	67.762266
1226.168332	73.047392	67.767271
1225.325205	61.847872	67.772276
1224.659079	67.899101	67.777281
1224.224787	71.546428	67.782286
1223.939803	67.860739	67.787290
1223.599189	75.708421	67.792295
1223.037968	70.824003	67.797300
1222.011663	76.024178	67.802305
1221.064833	70.884111	67.807310
1220.370489	69.353011	67.812314
1219.241183	66.484421	67.817319
1218.815605	73.121882	67.822324
1218.801210	72.357873	67.827329
1218.469625	76.491923	67.832334
1217.188635	67.803191	67.837338
1216.154906	76.855517	67.842343
1215.896860	69.688317	67.847348
1215.235778	73.139896	67.852353
1214.382892	73.717193	67.857358
1213.665179	74.689314	67.862362
1212.896515	77.005236	67.867367
1212.571702	73.387382	67.872372
1212.524958	71.272320	67.877377
1211.301241	71.022331	67.882382
1210.703243	62.865241	67.887386
1209.821093	74.870787	67.892391
1209.652313	70.504290	67.897396
1208.017275	76.706460	67.902401
1207.440757	80.171403	67.907406
1207.284927	71.109771	67.912410
1206.662218	76.792976	67.917415
1206.165190	74.230699	67.922420
1205.173834	73.297201	67.927425
1204.299995	74.626895	67.932430
1203.876831	67.725657	67.937434
1202.991047	80.327883	67.942439
1202.814243	68.856818	67.947444
1201.779028	70.371452	67.952449
1201.253623	72.905736	67.957454
1200.697093	72.861888	67.962458
1200.332811	71.888591	67.967463
1199.290757	71.358979	67.972468
1198.391309	72.375776	67.977473
1197.828705	62.901019	67.982478
1197.327060	58.056025	67.987482
1196.836283	67.834144	67.992487
1196.336967	69.413365	67.997492
1195.260200	73.651735	68.002497
1194.655552	70.079966	68.007502
1194.416133	64.592440	68.012506
1193.166918	64.046891	68.017511
1192.274869	64.482187	68.022516
1191.996463	67.713636	68.027521
1191.633954	78.387585	68.032526
1191.061089	66.471727	68.037530
1189.818925	77.668778	68.042535
1189.521556	66.743601	68.047540
1188.848634	72.158824	68.052545
1188.290078	65.933566	68.057550
1187.470985	71.509232	68.062554
1186.484579	73.844020	68.067559
1186.070567	67.457001	68.072564
1185.545552	68.245517	68.077569
1184.740142	68.654421	68.082574
1184.205924	73.446759	68.087578
1183.238573	81.137075	68.092583
1183.162064	71.916173	68.097588
1182.233273	81.492725	68.102593
1181.052765	77.717650	68.107598
1180.899339	71.897898	68.112602
1180.668883	69.651204	68.117607
1179.635057	68.686623	68.122612
1178.585967	77.807638	68.127617
1177.800223	67.128872	68.132622
1177.684543	72.505935	68.137626
1176.973220	74.024260	68.142631
1176.289671	61.441609	68.147636
1175.339175	66.675471	68.152641
1174.653240	74.502381	68.157646
1174.551046	68.773832	68.162650
1173.572452	76.814448	68.167655
1172.765254	64.495893	68.172660
1171.932080	70.408120	68.177665
1171.864395	77.665187	68.182670
1171.684109	72.776969	68.187674
1170.167736	76.386667	68.192679
1169.611302	66.437843	68.197684
1168.900292	70.652743	68.202689
1168.235757	67.238743	68.207694
1167.365716	65.647292	68.212698
1166.551608	67.584095	68.217703
1166.077157	62.731627	68.222708
1165.856270	67.778487	68.227713
1165.186138	69.757047	68.232718
1164.725758	56.023991	68.237722
1163.690154	69.741309	68.242727
1163.203004	61.768457	68.247732
1162.187976	68.567482	68.252737
1161.016173	72.992870	68.257742
1161.008006	67.151596	68.262746
1160.165045	76.810695	68.267751
1160.395192	67.908460	68.272756
1159.134253	68.180086	68.277761
1158.176286	71.235768	68.282766
1157.654214	67.100514	68.287770
1157.045770	76.984091	68.292775
1156.487329	68.913765	68.297780
1155.570494	67.477996	68.302785
1154.928676	70.760942	68.307790
1154.985913	60.298202	68.312794
1153.545624	70.101190	68.317799
1152.741142	64.410228	68.322804
1152.005019	67.026922	68.327809
1151.507035	66.207365	68.332814
1151.372981	61.542037	68.337818
1151.017165	64.717991	68.342823
1150.217997	71.507920	68.347828
1149.322158	63.803504	68.352833
1148.392109	73.137406	68.357838
1147.663852	62.004807	68.362842
1146.721030	68.954781	68.367847
1146.076180	71.921240	68.372852
1146.019562	63.671753	68.377857
1145.271017	67.138835	68.382862
1144.439089	65.194397	68.387866
1143.556375	66.247975	68.392871
1143.035694	65.061441	68.397876
1142.699884	64.058394	68.402881
1141.902213	68.030037	68.407886
1141.291321	56.866161	68.412890
1140.124903	72.039337	68.417895
1139.626796	66.498347	68.422900
1139.279139	69.165221	68.427905
1138.952957	64.773307	68.432910
1138.078757	59.815695	68.437914
1137.083190	67.234535	68.442919
1136.816253	71.276306	68.447924
1136.142172	67.641481	68.452929
1135.065240	64.747254	68.457934
1134.496432	62.574885	68.462938
1133.840173	67.377179	68.467943
1133.461402	53.197488	68.472948
1132.758847	54.200336	68.477953
1131.631253	62.856021	68.482958
1131.303303	53.093229	68.487962
1130.676942	61.088862	68.492967
1130.261654	61.858358	68.497972
1128.983204	62.974887	68.502977
1128.508652	60.954687	68.507982
1127.959281	53.608342	68.512986
1127.275782	60.578571	68.517991
1126.896727	65.500777	68.522996
1125.968677	67.056742	68.528001
1125.067387	71.576312	68.533006
1125.091200	62.650129	68.538010
1124.242106	60.175413	68.543015
1123.111005	59.956467	68.548020
1122.987446	53.725121	68.553025
1122.199491	73.592670	68.558030
1121.183328	55.218696	68.563034
1120.202874	65.394835	68.568039
1119.734945	60.221218	68.573044
1119.383936	62.447074	68.578049
1118.946799	74.003379	68.583054
1118.632803	58.056638	68.588058
1117.389053	66.407527	68.593063
1116.633730	55.522106	68.598068
1116.441321	63.518101	68.603073
1115.141297	65.822374	68.608078
1114.372873	49.951082	68.613082
1113.738169	60.758204	68.618087
1113.544062	55.799656	68.623092
1113.425991	59.906056	68.628097
1112.140647	64.865191	68.633102
1111.448930	62.655608	68.638106
1110.542542	63.235141	68.643111
1110.271195	65.957688	68.648116
1110.049595	63.518781	68.653121
1108.646453	61.226821	68.658126
1107.976795	64.143616	68.663130
1107.322459	58.763108	68.668135
1107.158776	63.640018	68.673140
1106.267095	61.239892	68.678145
1105.257328	65.660025	68.683150
1104.685669	49.352157	68.688154
1104.261595	71.006875	68.693159
1103.519266	64.771452	68.698164
1102.698914	65.545462	68.703169
1101.850402	63.017044	68.708174
1101.745695	63.664599	68.713178
1101.126891	66.000866	68.718183
1100.797966	63.416605	68.723188
1099.765831	70.101676	68.728193
1098.970793	72.316167	68.733198
1098.380335	62.785948	68.738202
1097.058974	62.882712	68.743207
1096.312994	59.751353	68.748212
1096.211310	58.310518	68.753217
1095.572279	75.798389	68.758222
1095.692223	56.029435	68.763226
1094.365374	66.964014	68.768231
1093.534750	64.743416	68.773236
1093.215788	57.032418	68.778241
1092.315145	62.132217	68.783246
1091.836689	64.974445	68.788250
1091.000104	66.217825	68.793255
1090.581856	64.196559	68.798260
1090.116823	56.027823	68.803265
1088.594794	58.979288	68.808270
1087.927563	53.394257	68.813274
1087.475427	63.595171	68.818279
1087.057059	58.043090	68.823284
1086.527699	57.279001	68.828289
1085.350172	74.437791	68.833294
1085.059532	65.465438	68.838298
1084.515329	66.700154	68.843303
1083.954631	56.280531	68.848308
1083.197181	63.801857	68.853313
1082.112290	67.372924	68.858318
1081.781162	60.740933	68.863322
1081.281648	65.724885	68.868327
1080.786702	63.789940	68.873332
1080.021324	62.227604	68.878337
1078.710117	66.457578	68.883342
1078.603549	63.740175	68.888346
1077.828891	60.726925	68.893351
1076.342737	64.189938	68.898356
1076.067718	66.985613	68.903361
1075.204616	65.687985	68.908366
1075.315183	60.725128	68.913370
1075.054626	60.867615	68.918375
1074.456052	63.788879	68.923380
1073.364588	55.059052	68.928385
1072.481345	61.941218	68.933390
1072.026821	58.441800	68.938394
1070.949789	65.145060	68.943399
1070.275890	61.093907	68.948404
1069.958260	56.415215	68.953409
1069.386922	63.448039	68.958414
1068.811443	53.153778	68.963418
1068.024025	58.997246	68.968423
1067.366051	62.519325	68.973428
1066.680028	53.882699	68.978433
1065.293321	59.026715	68.983438
1065.062494	55.769258	68.988442
1064.135977	52.518397	68.993447
1064.043119	53.889474	68.998452
1063.878538	50.886410	69.003457
1062.558451	62.589484	69.008462
1061.768507	59.269586	69.013466
1061.184132	55.669401	69.018471
1060.454119	57.209652	69.023476
1060.210727	58.716643	69.028481
1058.841777	57.549959	69.033486
1058.804701	52.668941	69.038490
1058.159072	59.289378	69.043495
1057.657684	66.618586	69.048500
1056.770179	57.749084	69.053505
1055.804907	66.718022	69.058510
1055.595785	56.684026	69.063514
1054.878749	58.480837	69.068519
1053.789667	63.766747	69.073524
1053.260704	62.591013	69.078529
1052.682637	66.879407	69.083534
1052.243048	61.964650	69.088538
1050.939654	64.067638	69.093543
1050.516916	69.651246	69.098548
1050.167904	55.451075	69.103553
1049.206145	64.756926	69.108558
1049.169896	52.416710	69.113562
1048.128241	59.194773	69.118567
1047.352515	57.435395	69.123572
1046.760113	55.531734	69.128577
1046.171406	53.624331	69.133582
1045.488398	57.347518	69.138586
1044.937791	64.172041	69.143591
1044.317274	63.272651	69.148596
1043.465376	57.095686	69.153601
1042.434333	73.322847	69.158606
1041.682573	57.035765	69.163610
1041.537863	59.984176	69.168615
1041.005416	60.433277	69.173620
1040.816249	54.355882	69.178625
1039.488228	65.986112	69.183630
1038.742929	58.565306	69.188634
1038.339107	64.111210	69.193639
1037.094944	71.060273	69.198644
1036.596658	58.899221	69.203649
1035.779335	63.131064	69.208654
1035.751596	58.395217	69.213658
1035.137020	65.944287	69.218663
1034.101767	66.907053	69.223668
1033.767997	68.799013	69.228673
1032.970477	65.406212	69.233678
1032.367086	62.857744	69.238682
1031.441709	68.765753	69.243687
1030.299576	59.697073	69.248692
1029.845726	55.383841	69.253697
1029.237411	64.663427	69.258702
1029.337996	58.626666	69.263706
1028.907548	57.982471	69.268711
1027.731015	52.629879	69.273716
1027.027391	49.225299	69.278721
1026.270912	62.570226	69.283726
1025.721246	56.285258	69.288730
1024.632056	63.939804	69.293735
1024.068036	68.235430	69.298740
1024.132180	55.931282	69.303745
1023.106864	60.590463	69.308750
1022.324856	54.277807	69.313754
1021.547231	59.339130	69.318759
1021.009512	56.092659	69.323764
1020.602805	49.322898	69.328769
1019.492149	64.104026	69.333774
1019.027692	52.320806	69.338778
1018.459440	57.473397	69.343783
1017.323242	58.822817	69.348788
1016.561181	57.729911	69.353793
1015.898415	60.806481	69.358798
1015.556008	57.223004	69.363802
1015.050167	56.627078	69.368807
1014.845664	61.422172	69.373812
1014.315490	57.960034	69.378817
1012.982173	67.440133	69.383822
1012.597920	58.969978	69.388826
1011.713335	60.392908	69.393831
1010.617055	67.778927	69.398836
1010.223885	56.687692	69.403841
1009.627477	68.543732	69.408846
1009.163118	61.008849	69.413850
1008.903426	63.133456	69.418855
1007.740133	70.883380	69.423860
1007.045097	60.207607	69.428865
1006.495822	68.347118	69.433870
1006.003024	65.423088	69.438874
1004.500915	56.963640	69.443879
1003.845791	59.723603	69.448884
1003.535558	58.347496	69.453889
1003.267499	53.298227	69.458894
1002.985921	57.555222	69.463898
1002.314070	58.352944	69.468903
1001.221725	56.162985	69.473908
1000.699568	61.120587	69.478913
999.931726	65.820812	69.483918
999.205675	54.391459	69.488922
998.568409	59.931931	69.493927
998.105211	62.489468	69.498932
997.561448	64.813818	69.503937
996.013565	67.488751	69.508942
995.701840	60.330136	69.513946
995.334090	62.938720	69.518951
994.744243	67.432428	69.523956
993.878200	50.865512	69.528961
992.894258	60.220637	69.533966
992.474664	62.547308	69.538970
992.411210	54.827217	69.543975
991.306213	55.162423	69.548980
990.382445	55.318983	69.553985
989.673877	59.691229	69.558990
989.346954	55.094457	69.563994
989.159888	62.704820	69.568999
988.063074	59.993600	69.574004
987.117215	59.508695	69.579009
986.519063	61.119449	69.584014
986.138529	60.785867	69.589018
985.236895	64.704708	69.594023
984.195440	56.380135	69.599028
984.114184	55.152101	69.604033
983.193975	54.333531	69.609038
982.915611	57.508216	69.614042
982.184201	58.679700	69.619047
981.070699	66.437479	69.624052
980.636114	56.149212	69.629057
980.249718	63.479053	69.634062
979.569478	52.321544	69.639066
978.945716	59.263372	69.644071
977.886362	63.232542	69.649076
977.571792	51.135323	69.654081
976.602448	59.650761	69.659086
975.546729	55.035916	69.664090
975.317638	57.445817	69.669095
974.647157	61.955511	69.674100
974.649895	63.205722	69.679105
973.499999	68.468224	69.684110
972.860429	59.054677	69.689114
972.364630	58.376736	69.694119
971.338707	60.184873	69.699124
970.626125	58.371318	69.704129
969.481122	61.857375	69.709134
969.204745	55.855369	69.714138
968.578318	63.800576	69.719143
968.114080	56.912244	69.724148
968.056130	56.388561	69.729153
966.935198	61.297945	69.734158
966.424872	53.488115	69.739162
966.093118	60.640525	69.744167
964.661303	65.503185	69.749172
964.082734	58.070069	69.754177
963.417774	61.744672	69.759182
962.883448	63.007803	69.764186
962.024507	58.949860	69.769191
961.048076	57.884775	69.774196
960.759535	52.338874	69.779201
960.220168	60.636084	69.784206
959.603655	62.309690	69.789210
959.451620	54.141647	69.794215
958.265684	67.651123	69.799220
957.959690	59.386149	69.804225
956.961075	67.770636	69.809230
956.066896	58.817084	69.814234
955.441891	58.490871	69.819239
954.796708	53.984174	69.824244
954.698716	54.556548	69.829249
953.422595	62.021664	69.834254
952.768360	59.452924	69.839258
952.639149	57.056105	69.844263
952.004188	56.942790	69.849268
951.080175	54.762337	69.854273
949.954514	62.078932	69.859278
949.672407	55.508556	69.864282
949.025969	58.530502	69.869287
948.489973	64.890663	69.874292
947.630912	54.944347	69.879297
946.644917	58.592769	69.884302
946.170702	53.279846	69.889306
946.123024	55.823307	69.894311
945.170704	60.597056	69.899316
944.428625	63.339331	69.904321
943.631015	57.136421	69.909326
943.326625	58.282540	69.914330
942.227454	62.172904	69.919335
941.486813	64.623213	69.924340
941.032411	49.796448	69.929345
940.741505	62.791330	69.934350
940.073661	59.212345	69.939354
939.065721	63.301082	69.944359
937.940830	74.563140	69.949364
937.648128	56.157726	69.954369
937.168525	54.710809	69.959374
936.227996	51.640428	69.964378
935.769154	55.980830	69.969383
934.901145	60.950902	69.974388
934.778451	48.706466	69.979393
934.003229	53.966124	69.984398
933.135496	53.572887	69.989402
932.262375	45.215251	69.994407
931.839393	57.296006	69.999412
931.550808	59.355829	70.004417
930.253819	65.252042	70.009422
929.621665	60.418422	70.014426
929.294485	54.566435	70.019431
928.707833	59.605275	70.024436
927.979752	58.027591	70.029441
926.686491	55.842831	70.034446
926.516673	58.541349	70.039450
926.313357	50.562824	70.044455
925.428094	65.632965	70.049460
924.519367	55.451710	70.054465
923.306735	58.975357	70.059470
923.072738	54.676048	70.064474
922.978447	50.914329	70.069479
921.854894	66.549101	70.074484
921.242022	53.657267	70.079489
920.785250	61.759986	70.084494
920.131269	63.382794	70.089498
919.496393	55.919230	70.094503
918.373048	57.009601	70.099508
918.039752	54.880233	70.104513
917.330887	54.054861	70.109518
916.829307	51.266294	70.114522
915.938458	55.035202	70.119527
914.838645	54.019734	70.124532
914.811614	56.941535	70.129537
914.156680	50.122993	70.134542
913.073903	58.063561	70.139546
912.674803	52.038520	70.144551
912.297984	57.551750	70.149556
911.526049	51.194957	70.154561
910.490604	51.978027	70.159566
909.760272	55.196262	70.164570
909.394269	47.434447	70.169575
908.723456	61.612588	70.174580
908.624453	42.670167	70.179585
907.405868	55.423171	70.184590
907.216016	54.387467	70.189594
906.361342	58.656828	70.194599
904.767991	58.547818	70.199604
904.498194	61.386829	70.204609
903.840621	59.261762	70.209614
903.524976	56.498799	70.214618
903.105492	54.104027	70.219623
901.775561	63.161004	70.224628
901.391043	48.741028	70.229633
900.908254	59.137643	70.234638
900.118197	54.278701	70.239642
899.487320	50.201835	70.244647
898.648506	59.051337	70.249652
898.154325	57.564170	70.254657
898.015234	58.426941	70.259662
896.989877	54.004422	70.264666
896.143974	45.700818	70.269671
895.040852	60.483931	70.274676
895.089432	53.072453	70.279681
893.920451	55.985187	70.284686
892.792727	59.061667	70.289690
892.775070	55.850731	70.294695
892.123448	61.543320	70.299700
891.855211	47.786091	70.304705
891.405037	54.102634	70.309710
890.118344	57.991323	70.314714
889.445107	54.269709	70.319719
888.782795	59.432562	70.324724
888.737019	51.679708	70.329729
887.474305	51.533856	70.334734
886.851224	52.481542	70.339738
886.709136	51.078690	70.344743
885.130752	60.272988	70.349748
884.723643	54.719162	70.354753
884.030025	55.862581	70.359758
883.444759	55.988958	70.364762
883.277538	57.934851	70.369767
882.156617	60.138191	70.374772
881.385465	55.333019	70.379777
880.742355	59.374748	70.384782
880.058479	67.499427	70.389786
880.386024	53.639487	70.394791
879.214604	58.574286	70.399796
878.426680	55.014433	70.404801
877.691098	62.719982	70.409806
876.854828	52.405793	70.414810
876.372063	48.005736	70.419815
875.440558	52.356720	70.424820
875.042755	51.357271	70.429825
874.489884	58.283102	70.434830
873.589100	62.007874	70.439834
872.824517	60.347706	70.444839
872.258130	60.474235	70.449844
872.138932	51.085139	70.454849
871.394368	59.424480	70.459854
870.345309	67.641978	70.464858
869.523596	48.984901	70.469863
868.768402	58.563851	70.474868
868.654022	62.969288	70.479873
867.486135	59.600803	70.484878
866.541472	57.306974	70.489882
866.088665	55.950424	70.494887
865.674304	46.586235	70.499892
865.596720	52.305731	70.504897
864.688440	61.893281	70.509902
863.868092	58.586177	70.514906
863.347103	46.425652	70.519911
862.829820	59.043395	70.524916
861.957878	58.877936	70.529921
861.139072	51.399515	70.534926
860.562077	59.606530	70.539930
860.653470	48.714186	70.544935
858.874794	54.196659	70.549940
858.033674	49.544560	70.554945
857.765242	59.754094	70.559950
857.145050	55.287604	70.564954
856.489910	57.880445	70.569959
855.611040	49.045935	70.574964
855.289083	46.711344	70.579969
855.180242	56.384536	70.584974
853.837578	56.278235	70.589978
853.285518	46.596918	70.594983
852.571760	47.484928	70.599988
852.067501	45.390668	70.604993
850.931195	48.960543	70.609998
849.781154	52.889000	70.615002
849.387468	44.522898	70.620007
848.839093	54.713909	70.625012
848.645613	47.514432	70.630017
848.502838	58.995498	70.635022
848.054789	51.760845	70.640026
846.864395	53.609401	70.645031
846.284630	61.141919	70.650036
845.456747	53.294361	70.655041
844.315020	53.376856	70.660046
843.747459	48.635487	70.665050
843.589774	48.608658	70.670055
842.572467	52.445026	70.675060
841.982322	49.686344	70.680065
841.329730	57.208375	70.685070
840.900355	53.962050	70.690074
840.366742	51.137599	70.695079
838.905462	53.612755	70.700084
838.673525	47.651010	70.705089
838.417536	55.808507	70.710094
837.307779	57.768813	70.715098
836.437171	48.384213	70.720103
835.515750	60.186342	70.725108
835.228074	53.110669	70.730113
834.769441	52.676001	70.735118
834.438325	52.509620	70.740122
833.387543	45.158026	70.745127
832.589976	58.463787	70.750132
832.212862	45.526583	70.755137
831.732987	48.146723	70.760142
830.711655	52.633446	70.765146
829.965728	44.148375	70.770151
829.105008	58.918151	70.775156
828.896461	45.446332	70.780161
828.490752	56.627047	70.785166
827.259575	61.615536	70.790170
826.939183	53.289807	70.795175
826.234706	59.542760	70.800180
825.641073	50.393197	70.805185
824.430697	58.626922	70.810190
823.660584	60.798100	70.815194
823.668223	51.518132	70.820199
823.074722	52.726054	70.825204
822.392190	49.321336	70.830209
821.702807	50.721141	70.835214
820.989992	57.246659	70.840218
820.541612	53.749473	70.845223
819.271556	63.188042	70.850228
818.798121	54.259044	70.855233
818.449652	49.441805	70.860238
817.392770	58.335502	70.865242
817.077841	48.588062	70.870247
816.255456	58.097294	70.875252
815.997468	53.223073	70.880257
814.951834	48.204575	70.885262
813.951565	56.303931	70.890266
813.452232	46.961166	70.895271
812.884674	51.709976	70.900276
812.501214	55.910661	70.905281
811.594327	50.892154	70.910286
810.671993	55.025655	70.915290
810.289659	50.710552	70.920295
809.476537	52.445452	70.925300
809.414150	48.825322	70.930305
808.215905	48.812751	70.935310
807.331869	61.291763	70.940314
807.490921	48.895266	70.945319
806.497815	56.143500	70.950324
805.357361	53.543394	70.955329
804.681152	52.471581	70.960334
804.342104	57.612952	70.965338
804.099125	48.631506	70.970343
802.929722	52.107322	70.975348
802.121170	54.421819	70.980353
801.704157	47.510249	70.985358
801.015547	57.193730	70.990362
800.787339	56.219335	70.995367
799.541977	55.794796	71.000372
799.213443	52.464618	71.005377
798.754886	53.335672	71.010382
797.706572	51.335918	71.015386
797.092615	47.130231	71.020391
796.019804	52.508261	71.025396
795.656881	58.519188	71.030401
795.518112	48.511897	71.035406
794.530986	53.649204	71.040410
793.748475	45.100585	71.045415
792.999842	54.038256	71.050420
792.566669	51.815997	71.055425
791.531770	54.977090	71.060430
790.765122	55.274291	71.065434
790.552534	51.116674	71.070439
790.009795	57.455850	71.075444
789.374643	49.462517	71.080449
788.462849	57.068399	71.085454
787.897172	52.301514	71.090458
787.702430	50.866050	71.095463
786.407208	55.497318	71.100468
785.453092	57.208939	71.105473
785.105959	46.157756	71.110478
784.458741	56.479628	71.115482
784.221050	47.598270	71.120487
783.126889	53.862804	71.125492
782.380032	54.617330	71.130497
781.954214	55.558869	71.135502
780.969654	58.814456	71.140506
780.949875	55.742635	71.145511
780.002827	64.779712	71.150516
779.382252	50.884635	71.155521
779.013459	44.780684	71.160526
777.580995	44.247171	71.165530
776.797998	48.976668	71.170535
775.972769	50.139491	71.175540
775.599470	55.835100	71.180545
775.426765	50.789613	71.185550
774.720596	58.761736	71.190554
774.566618	45.798486	71.195559
773.475806	57.640211	71.200564
772.804093	54.331556	71.205569
772.326280	54.759399	71.210574
771.139227	58.110305	71.215578
771.016132	57.863506	71.220583
770.099149	61.737548	71.225588
769.158186	53.608401	71.230593
768.399547	51.876358	71.235598
767.852707	55.264114	71.240602
767.774008	49.736880	71.245607
766.655955	55.208857	71.250612
765.471559	55.846965	71.255617
765.148865	51.850384	71.260622
764.301369	58.963487	71.265626
764.280957	63.054340	71.270631
764.008380	57.502776	71.275636
762.839464	57.032969	71.280641
762.299675	51.009860	71.285646
761.290875	55.256492	71.290650
761.043317	53.950865	71.295655
759.843356	65.850980	71.300660
759.109456	55.842244	71.305665
758.656792	56.663481	71.310670
758.236511	54.902802	71.315674
757.316491	61.647406	71.320679
756.515120	60.923542	71.325684
756.294280	52.616673	71.330689
755.856754	52.825214	71.335694
754.847830	55.472827	71.340698
754.095839	55.561123	71.345703
753.469271	54.025679	71.350708
752.915098	43.203012	71.355713
752.472663	40.950698	71.360718
751.121136	57.023927	71.365722
750.750695	44.856820	71.370727
750.193847	62.273263	71.375732
749.711527	52.295442	71.380737
748.858289	53.379154	71.385742
748.030028	55.669997	71.390746
747.661201	51.605070	71.395751
747.215804	56.963653	71.400756
746.154774	58.091487	71.405761
745.335787	48.214582	71.410766
744.732265	51.482055	71.415770
744.615374	44.350827	71.420775
743.737617	54.745679	71.425780
742.740406	55.270415	71.430785
742.464314	48.913590	71.435790
741.631751	55.920240	71.440794
741.213228	50.956473	71.445799
739.994538	53.071359	71.450804
739.289781	51.742334	71.455809
738.747683	51.216894	71.460814
738.420716	57.507531	71.465818
737.945297	43.953644	71.470823
736.967625	55.217543	71.475828
736.155358	56.310506	71.480833
735.877360	47.282610	71.485838
734.668178	51.796122	71.490842
734.258152	49.480302	71.495847
733.750644	53.585627	71.500852
733.309910	50.088820	71.505857
732.645275	49.365271	71.510862
731.235683	55.183303	71.515866
730.688438	46.395399	71.520871
730.410626	49.495896	71.525876
730.096171	54.828900	71.530881
729.366820	45.604787	71.535886
728.305045	55.505392	71.540890
728.048524	40.606203	71.545895
727.094319	52.358378	71.550900
726.319261	57.264824	71.555905
725.821244	55.708918	71.560910
725.130657	55.325396	71.565914
724.527625	50.548707	71.570919
723.356976	50.733634	71.575924
722.535846	48.027531	71.580929
722.460452	46.208793	71.585934
721.932726	50.651654	71.590938
721.787687	44.067386	71.595943
720.870237	54.099554	71.600948
720.063515	55.609534	71.605953
719.133238	46.059446	71.610958
717.837162	57.295201	71.615962
717.253676	45.256643	71.620967
716.963996	47.792902	71.625972
716.558477	53.599302	71.630977
716.411682	50.303280	71.635982
715.311563	55.873347	71.640986
714.465714	43.605329	71.645991
713.773983	45.661552	71.650996
713.361547	58.245264	71.656001
712.796418	52.499017	71.661006
711.428980	56.709731	71.666010
711.072781	51.628813	71.671015
710.521785	53.602705	71.676020
710.221066	55.538323	71.681025
709.491689	48.993481	71.686030
708.383683	52.347597	71.691034
708.046431	45.210460	71.696039
707.265076	52.385583	71.701044
706.369904	50.493949	71.706049
705.817881	44.758237	71.711054
705.066241	47.819065	71.716058
705.062870	42.210459	71.721063
704.002925	42.185379	71.726068
703.038253	46.503850	71.731073
702.621760	42.361369	71.736078
701.760572	46.018385	71.741082
701.422249	48.584468	71.746087
700.351078	47.644962	71.751092
699.727650	49.155723	71.756097
699.252226	56.260058	71.761102
698.816261	53.759139	71.766106
698.403978	50.689898	71.771111
697.371316	63.301411	71.776116
696.537228	49.489253	71.781121
696.291701	45.283278	71.786126
695.258720	48.489833	71.791130
694.504469	45.681628	71.796135
693.798835	52.228105	71.801140
693.237933	52.590345	71.806145
692.833666	52.888219	71.811150
692.313543	55.275094	71.816154
691.454521	49.553576	71.821159
690.680534	56.856842	71.826164
690.357556	59.133477	71.831169
689.735763	45.227597	71.836174
688.338649	58.821242	71.841178
688.021807	50.569098	71.846183
687.442783	48.690208	71.851188
686.810412	52.690843	71.856193
686.036027	53.821943	71.861198
685.094450	51.833627	71.866202
684.875474	51.411288	71.871207
684.505471	51.864558	71.876212
683.672970	53.730316	71.881217
682.826505	54.462886	71.886222
682.006829	51.778643	71.891226
681.870360	56.432023	71.896231
681.244014	47.005444	71.901236
680.006842	56.248016	71.906241
679.883162	48.960179	71.911246
678.904634	52.230610	71.916250
677.912649	44.311487	71.921255
677.146881	53.523147	71.926260
676.858166	47.911094	71.931265
676.636381	40.615229	71.936270
675.394359	60.365871	71.941274
674.667380	54.184936	71.946279
674.103853	46.254356	71.951284
673.652774	44.476521	71.956289
673.249211	49.989298	71.961294
671.799661	54.711427	71.966298
671.311870	46.631592	71.971303
670.973270	45.392514	71.976308
670.233851	52.523121	71.981313
670.014393	49.768533	71.986318
668.591822	45.253257	71.991322
668.320756	53.805818	71.996327
667.702801	48.482740	72.001332
667.175908	51.980878	72.006337
666.644748	44.604968	72.011342
665.549458	49.032563	72.016346
665.247340	45.805436	72.021351
664.468250	45.579529	72.026356
663.253039	51.503835	72.031361
662.889284	40.720264	72.036366
662.285653	51.511452	72.041370
662.096863	46.284037	72.046375
660.829389	44.100047	72.051380
660.057951	47.182964	72.056385
659.615330	53.717526	72.061390
659.014990	55.208851	72.066394
658.570183	45.862182	72.071399
657.456465	46.724052	72.076404
656.773660	48.073967	72.081409
656.822626	47.397649	72.086414
655.958844	51.703225	72.091418
655.306822	48.538129	72.096423
654.208321	48.678482	72.101428
653.634772	52.344902	72.106433
653.278943	50.028352	72.111438
652.035928	53.640535	72.116442
651.866983	54.285720	72.121447
651.264921	41.717134	72.126452
650.693720	54.848102	72.131457
649.950203	45.438618	72.136462
648.718038	58.047218	72.141466
648.391933	55.301731	72.146471
648.018572	51.701172	72.151476
647.249902	54.414643	72.156481
646.633068	49.395747	72.161486
645.687702	57.273522	72.166490
645.273092	48.065550	72.171495
644.537874	47.799545	72.176500
643.503944	46.218618	72.181505
643.151417	49.466639	72.186510
642.601885	52.110520	72.191514
642.246240	52.036381	72.196519
640.861972	45.654207	72.201524
640.557890	47.960952	72.206529
639.952139	45.392468	72.211534
639.127294	55.882999	72.216538
638.828323	43.021719	72.221543
638.242254	45.939501	72.226548
637.279948	47.989949	72.231553
636.703322	44.659887	72.236558
635.537060	58.527450	72.241562
635.086796	56.946612	72.246567
634.588788	41.636472	72.251572
634.287487	47.800020	72.256577
633.646795	42.486884	72.261582
632.392311	44.549172	72.266586
631.754668	44.535715	72.271591
631.924928	44.587558	72.276596
630.536955	43.357913	72.281601
629.855415	42.376886	72.286606
629.180118	50.516005	72.291610
628.796480	45.229740	72.296615
627.973192	42.935602	72.301620
627.012009	44.632636	72.306625
626.631652	35.624227	72.311630
626.103924	51.149978	72.316634
625.486360	46.763567	72.321639
624.264321	52.409855	72.326644
623.543998	51.416082	72.331649
623.137390	44.427205	72.336654
622.796693	49.023223	72.341658
622.465802	46.193348	72.346663
621.882753	45.879461	72.351668
620.229418	57.422890	72.356673
620.130651	45.288246	72.361678
619.698720	49.439899	72.366682
619.101688	45.564308	72.371687
618.039007	41.401757	72.376692
617.189812	51.836243	72.381697
617.040349	53.366156	72.386702
615.691559	46.860075	72.391706
615.068112	47.743228	72.396711
614.722692	44.666509	72.401716
614.150823	46.036614	72.406721
613.974914	46.779104	72.411726
613.018185	51.162575	72.416730
612.193353	48.874996	72.421735
611.938222	47.688866	72.426740
610.666491	44.609867	72.431745
609.961754	37.444550	72.436750
609.259501	46.952034	72.441754
608.801705	50.723030	72.446759
608.621442	48.785381	72.451764
607.386724	49.105146	72.456769
606.930564	44.834960	72.461774
606.344316	49.468511	72.466778
605.636555	46.299692	72.471783
604.672638	38.138016	72.476788
603.647041	52.864700	72.481793
603.383793	48.525942	72.486798
602.594426	48.926167	72.491802
602.641641	50.874189	72.496807
602.199237	48.071539	72.501812
600.878269	47.919341	72.506817
600.429186	37.912628	72.511822
599.397012	54.605254	72.516826
598.350401	44.898711	72.521831
597.761529	43.656928	72.526836
597.017887	49.111913	72.531841
597.129951	40.704749	72.536846
596.414531	48.594796	72.541850
596.178785	47.176920	72.546855
595.019659	46.417050	72.551860
594.345507	48.128304	72.556865
593.720636	42.030488	72.561870
593.141035	45.343066	72.566874
592.443542	47.767670	72.571879
591.434205	49.757817	72.576884
590.887743	48.682746	72.581889
590.826457	50.980787	72.586894
589.708467	54.814361	72.591898
589.181693	49.298588	72.596903
588.695054	44.875565	72.601908
587.386810	53.497130	72.606913
586.693010	51.608161	72.611918
586.270919	57.104978	72.616922
585.719393	60.018848	72.621927
585.155424	59.506387	72.626932
584.193055	54.170381	72.631937
583.724133	49.545839	72.636942
582.933612	56.200479	72.641946
582.714643	51.681205	72.646951
582.380959	43.327691	72.651956
581.407106	51.088593	72.656961
580.787170	48.126567	72.661966
579.494618	50.417297	72.666970
578.569089	52.455601	72.671975
578.181984	45.212891	72.676980
577.523777	56.932154	72.681985
577.343872	52.658971	72.686990
576.825016	58.738907	72.691994
575.608464	52.393136	72.696999
574.987756	53.116591	72.702004
574.377669	56.940235	72.707009
574.395963	50.082385	72.712014
573.144415	55.324964	72.717018
572.439403	51.346736	72.722023
571.991712	48.038731	72.727028
571.013731	55.357171	72.732033
570.387178	52.588590	72.737038
569.343587	48.547598	72.742042
568.878087	50.575709	72.747047
568.662863	49.082028	72.752052
567.734854	46.944941	72.757057
567.764340	46.647041	72.762062
566.458970	55.547281	72.767066
565.750923	41.366610	72.772071
565.318574	48.266975	72.777076
564.844355	54.863352	72.782081
564.256627	45.299778	72.787086
563.119249	54.081796	72.792090
562.639496	48.650004	72.797095
562.135562	50.152802	72.802100
560.714259	51.603029	72.807105
560.617566	45.679712	72.812110
559.939173	53.453484	72.817114
559.538763	46.026816	72.822119
558.990222	43.963330	72.827124
557.897353	49.735728	72.832129
557.615035	42.862689	72.837134
556.904095	49.225534	72.842138
555.779888	50.521206	72.847143
554.799645	41.636752	72.852148
554.167806	53.799671	72.857153
554.097076	52.483248	72.862158
553.992724	52.602483	72.867162
552.862577	51.175693	72.872167
552.097421	53.084382	72.877172
551.167688	61.155240	72.882177
550.865049	49.819483	72.887182
549.905057	52.386838	72.892186
549.085549	51.891436	72.897191
548.895870	55.678080	72.902196
548.212883	56.886127	72.907201
547.702883	48.475548	72.912206
546.522562	53.224243	72.917210
545.894064	45.529558	72.922215
545.644729	46.269556	72.927220
544.626366	53.794710	72.932225
544.097156	50.996438	72.937230
543.347928	56.692027	72.942234
543.228831	54.411901	72.947239
542.690086	54.931495	72.952244
541.686812	55.715899	72.957249
540.976672	52.328280	72.962254
540.158459	56.759099	72.967258
538.891578	53.531130	72.972263
538.523907	48.571925	72.977268
538.045641	57.107033	72.982273
537.838950	43.997689	72.987278
537.137222	53.883577	72.992282
535.833831	57.751438	72.997287
535.316114	49.968144	73.002292
534.945600	51.187919	73.007297
534.427625	49.368729	73.012302
533.459703	53.605776	73.017306
532.249029	50.698444	73.022311
532.070155	46.809882	73.027316
531.241399	51.827433	73.032321
531.464709	41.850821	73.037326
530.601275	46.203687	73.042330
529.555363	50.470505	73.047335
529.352473	46.470652	73.052340
528.268136	49.573487	73.057345
527.540340	47.057592	73.062350
526.746889	53.070889	73.067354
526.001855	48.223840	73.072359
525.774088	40.470059	73.077364
524.992301	49.864072	73.082369
524.404983	45.510720	73.087374
523.840796	49.424832	73.092378
523.235812	52.046030	73.097383
522.289533	41.553991	73.102388
521.365114	52.397876	73.107393
520.755347	52.383160	73.112398
520.651588	53.498941	73.117402
519.672131	53.707122	73.122407
518.866309	44.506315	73.127412
517.959229	48.911870	73.132417
517.766583	44.883578	73.137422
517.111605	49.671598	73.142426
516.502553	56.647430	73.147431
515.588613	53.527253	73.152436
514.822088	58.443433	73.157441
514.718574	51.152404	73.162446
514.489601	46.492808	73.167450
513.066741	52.907576	73.172455
512.477478	37.968416	73.177460
511.725816	51.943428	73.182465
510.977164	48.990888	73.187470
509.812220	52.571776	73.192474
509.257821	47.314316	73.197479
509.162288	42.165108	73.202484
508.734463	46.811285	73.207489
507.973805	37.947068	73.212494
507.388989	49.091668	73.217498
506.566322	49.440457	73.222503
506.096794	49.852837	73.227508
504.784533	56.473920	73.232513
504.112257	52.921008	73.237518
503.805581	57.762355	73.242522
503.220605	56.185659	73.247527
502.968740	43.555030	73.252532
501.619453	51.265381	73.257537
501.325081	52.936656	73.262542
500.805415	47.069691	73.267546
499.865402	49.589725	73.272551
499.338455	45.483806	73.277556
498.844691	51.725334	73.282561
497.988360	44.390239	73.287566
497.048966	55.282250	73.292570
496.006848	51.095977	73.297575
495.859214	48.817248	73.302580
495.367857	55.141973	73.307585
494.976176	48.388868	73.312590
493.614688	48.105987	73.317594
492.945642	50.877747	73.322599
493.038637	39.075281	73.327604
491.922916	49.959110	73.332609
490.895315	45.486676	73.337614
490.164494	51.567275	73.342618
489.463204	52.497554	73.347623
489.769941	40.965387	73.352628
489.165832	53.005623	73.357633
488.226966	44.013683	73.362638
487.633267	44.001147	73.367642
486.939178	53.217196	73.372647
485.716387	38.984529	73.377652
485.035212	40.398883	73.382657
484.179041	42.851948	73.387662
484.123726	46.688149	73.392666
483.415778	47.239443	73.397671
482.448442	44.950960	73.402676
481.835457	58.116987	73.407681
481.623819	42.740778	73.412686
481.070584	42.696565	73.417690
479.766233	46.354868	73.422695
479.401494	45.238256	73.427700
478.163745	50.680528	73.432705
478.137185	48.682133	73.437710
477.854234	43.021890	73.442714
476.881877	39.742305	73.447719
476.352040	37.675860	73.452724
475.550832	44.759580	73.457729
474.666921	50.984421	73.462734
473.567883	46.094444	73.467738
472.943817	53.225639	73.472743
472.954819	40.084784	73.477748
472.118747	48.687939	73.482753
471.594412	45.116200	73.487758
470.926455	43.309883	73.492762
470.153386	45.532092	73.497767
469.614902	55.369906	73.502772
468.736072	53.336987	73.507777
467.707782	43.370552	73.512782
467.319957	52.544116	73.517786
466.649219	51.271253	73.522791
466.241093	45.443297	73.527796
465.829483	55.407554	73.532801
465.146282	53.240965	73.537806
464.564776	51.605379	73.542810
463.572822	52.187736	73.547815
462.846001	48.717645	73.552820
461.877564	56.977620	73.557825
461.359297	52.930251	73.562830
460.966112	52.934659	73.567834
460.059897	50.426712	73.572839
459.401319	35.732008	73.577844
458.545782	52.308211	73.582849
458.286188	45.333797	73.587854
457.990317	47.563558	73.592858
457.029829	50.015907	73.597863
456.360845	43.070452	73.602868
455.696804	54.614039	73.607873
454.948879	49.791130	73.612878
454.455369	48.469533	73.617882
453.751474	55.479410	73.622887
453.320280	41.992694	73.627892
452.378903	49.549765	73.632897
451.673830	37.954885	73.637902
450.867869	51.839210	73.642906
450.244501	50.032101	73.647911
450.018157	43.410361	73.652916
448.611821	43.737048	73.657921
448.189170	45.157530	73.662926
447.765466	51.886220	73.667930
447.154203	52.165076	73.672935
446.812086	47.204971	73.677940
445.484430	50.805504	73.682945
444.920391	43.855947	73.687950
444.446157	47.393041	73.692954
443.363681	47.459971	73.697959
443.012987	48.089972	73.702964
442.076099	58.227815	73.707969
441.853454	52.206304	73.712974
441.571013	46.508138	73.717978
440.264124	49.637008	73.722983
439.920004	48.356266	73.727988
438.909985	55.558426	73.732993
438.624844	49.013864	73.737998
437.439700	51.982988	73.743002
436.769061	48.929733	73.748007
436.153713	45.579086	73.753012
435.590469	55.416118	73.758017
435.410029	49.151341	73.763022
434.905502	51.026420	73.768026
433.788505	49.100850	73.773031
433.673501	45.714635	73.778036
432.166281	53.234140	73.783041
431.672476	45.682036	73.788046
431.110123	47.396018	73.793050
430.426589	51.562554	73.798055
430.198068	39.016538	73.803060
428.764671	55.924523	73.808065
428.253842	38.943352	73.813070
427.980510	43.599614	73.818074
427.462138	52.273586	73.823079
426.757276	49.213172	73.828084
425.616586	49.902822	73.833089
425.152567	45.482542	73.838094
424.600612	43.846989	73.843098
423.743499	47.683215	73.848103
423.364060	33.207403	73.853108
422.519705	49.873290	73.858113
422.173256	46.626457	73.863118
421.483968	47.832387	73.868122
420.574238	54.138630	73.873127
419.734229	46.316841	73.878132
419.200245	53.343805	73.883137
419.090037	45.799967	73.888142
417.981187	42.239380	73.893146
417.151936	43.489690	73.898151
416.524734	45.251855	73.903156
415.887910	52.941759	73.908161
415.294237	46.569367	73.913166
414.582845	53.498445	73.918170
413.649188	49.761707	73.923175
413.293471	45.136515	73.928180
412.656684	34.248290	73.933185
412.094975	40.049641	73.938190
411.253303	42.246529	73.943194
410.513790	49.159586	73.948199
410.363077	36.850336	73.953204
409.630162	51.082573	73.958209
408.663325	50.689544	73.963214
408.404925	40.816504	73.968218
407.595772	49.412232	73.973223
406.696676	33.566855	73.978228
405.767251	46.991462	73.983233
405.202978	44.358085	73.988238
404.999290	42.469921	73.993242
404.248178	45.991217	73.998247
403.220137	40.717801	74.003252
402.557610	44.792685	74.008257
402.420612	45.098479	74.013262
401.893890	44.316774	74.018266
400.281993	47.776542	74.023271
400.132586	32.272177	74.028276
399.476737	40.468157	74.033281
398.768333	43.613641	74.038286
397.965378	43.522508	74.043290
396.699558	47.491680	74.048295
396.640826	48.523018	74.053300
396.434227	50.446822	74.058305
396.042900	48.539673	74.063310
395.212453	51.803955	74.068314
394.043749	48.361726	74.073319
394.090025	41.731246	74.078324
392.311946	55.439335	74.083329
391.886814	41.104848	74.088334
391.476346	47.202226	74.093338
390.548667	46.394533	74.098343
390.852061	35.271335	74.103348
389.308426	38.108371	74.108353
388.669582	47.197358	74.113358
388.264735	41.085047	74.118362
387.885107	43.120003	74.123367
387.278869	38.047461	74.128372
385.979126	44.735984	74.133377
385.477975	41.774009	74.138382
385.178761	40.654855	74.143386
384.137370	44.085219	74.148391
383.280796	43.162118	74.153396
382.623002	43.921491	74.158401
382.482688	40.011034	74.163406
382.075125	38.041821	74.168410
380.917389	42.876871	74.173415
380.225620	33.323640	74.178420
379.766771	41.702696	74.183425
379.140568	35.414353	74.188430
378.182717	40.275896	74.193434
376.991578	48.181873	74.198439
377.094134	45.886939	74.203444
376.512774	48.928604	74.208449
376.004284	39.833442	74.213454
375.102184	41.838121	74.218458
374.276056	52.349411	74.223463
373.909305	42.968309	74.228468
372.928948	49.847216	74.233473
372.161382	51.991307	74.238478
371.562658	39.966348	74.243482
370.555497	46.076818	74.248487
370.505505	41.298835	74.253492
370.283431	53.133122	74.258497
369.073725	44.778914	74.263502
368.594241	46.780901	74.268506
367.885253	39.930163	74.273511
367.012813	39.099483	74.278516
365.934916	43.051336	74.283521
365.600328	44.918268	74.288526
365.339086	41.334591	74.293530
364.728019	49.293210	74.298535
364.078148	43.746655	74.303540
363.298403	43.407406	74.308545
362.458212	48.142973	74.313550
361.460871	49.981486	74.318554
360.575371	45.519583	74.323559
360.148658	47.946824	74.328564
359.707687	50.969274	74.333569
359.718158	46.662625	74.338574
359.428625	43.321578	74.343578
358.024190	50.838933	74.348583
357.822164	47.160663	74.353588
356.513734	47.662611	74.358593
355.609330	47.792664	74.363598
355.247541	48.891224	74.368602
354.732741	47.625081	74.373607
353.775795	44.578058	74.378612
352.755252	53.243761	74.383617
352.233377	46.027314	74.388622
351.750823	45.355276	74.393626
351.116357	48.693993	74.398631
350.837833	47.238808	74.403636
349.853045	48.723663	74.408641
348.827861	50.870971	74.413646
348.646512	46.161232	74.418650
348.087501	48.275245	74.423655
348.142127	40.713033	74.428660
347.032409	45.524675	74.433665
345.991027	46.294729	74.438670
345.072457	42.659697	74.443674
343.717642	45.044044	74.448679
343.850420	46.352367	74.453684
343.089273	49.523618	74.458689
342.676089	46.982872	74.463694
342.450387	43.991200	74.468698
341.522318	49.224904	74.473703
341.085987	36.040248	74.478708
339.982959	40.071809	74.483713
339.047657	45.786060	74.488718
338.382969	33.218121	74.493722
337.144015	35.629737	74.498727
337.260644	44.096853	74.503732
336.819712	49.644005	74.508737
336.366445	51.020499	74.513742
335.709001	42.325981	74.518746
334.901704	52.470002	74.523751
334.336292	47.067690	74.528756
333.389634	50.274818	74.533761
332.387157	45.391599	74.538766
332.041211	40.496785	74.543770
331.631159	48.708800	74.548775
331.268329	41.596324	74.553780
330.088318	45.001493	74.558785
329.191378	47.681880	74.563790
328.949068	40.233228	74.568794
328.167993	47.157657	74.573799
327.407977	41.335357	74.578804
326.882860	44.740228	74.583809
326.351183	53.146673	74.588814
325.821651	37.917371	74.593818
324.559417	41.796117	74.598823
324.154705	33.301024	74.603828
323.613318	35.429578	74.608833
322.981838	41.857077	74.613838
322.104900	40.866281	74.618842
321.150545	43.510089	74.623847
320.948014	46.240650	74.628852
320.599379	42.994184	74.633857
319.333814	45.197162	74.638862
318.996613	39.460440	74.643866
318.225846	48.150995	74.648871
318.066953	42.841593	74.653876
316.710703	46.571326	74.658881
316.131313	44.549087	74.663886
315.839057	41.150133	74.668890
314.738680	50.125038	74.673895
313.707849	43.932743	74.678900
313.045608	48.852851	74.683905
312.844915	46.344475	74.688910
312.553849	41.153911	74.693914
311.871285	42.281527	74.698919
311.223718	44.748707	74.703924
310.310087	48.814750	74.708929
309.887249	48.081163	74.713934
309.010127	42.558233	74.718938
308.100099	49.835959	74.723943
307.436295	47.281550	74.728948
306.994682	49.063046	74.733953
306.438823	41.101401	74.738958
305.789596	31.298568	74.743962
304.729212	48.984501	74.748967
304.154099	46.736079	74.753972
304.058751	44.005909	74.758977
302.998293	51.941551	74.763982
302.249608	38.431376	74.768986
301.740327	41.463143	74.773991
301.232102	44.133621	74.778996
300.276103	45.784217	74.784001
299.196655	47.946501	74.789006
298.851851	42.687234	74.794010
298.245946	52.542119	74.799015
298.093229	44.087285	74.804020
297.333786	51.859831	74.809025
296.400498	51.261226	74.814030
295.507523	37.770900	74.819034
294.927854	44.956547	74.824039
294.722488	50.805201	74.829044
293.912778	44.588710	74.834049
292.914127	47.941334	74.839054
292.897454	42.139333	74.844058
292.101842	47.932258	74.849063
291.017757	47.335614	74.854068
290.237018	41.729519	74.859073
289.773754	46.753533	74.864078
289.280266	46.928498	74.869082
288.408979	55.001151	74.874087
287.690337	43.036337	74.879092
287.079815	43.901740	74.884097
286.680612	49.467478	74.889102
286.119935	46.461398	74.894106
284.810650	49.926618	74.899111
284.511727	45.617251	74.904116
283.868635	48.913203	74.909121
283.599149	49.413587	74.914126
282.470882	41.749772	74.919130
281.611923	48.503701	74.924135
281.136388	30.168678	74.929140
280.891391	46.687006	74.934145
279.858457	39.132577	74.939150
279.434080	35.936040	74.944154
278.408892	46.307190	74.949159
278.295733	37.240507	74.954164
277.174844	43.168862	74.959169
276.304238	42.916665	74.964174
276.036521	46.936529	74.969178
275.228873	42.706679	74.974183
274.876368	47.974814	74.979188
274.100416	40.196497	74.984193
273.692369	41.926915	74.989198
272.999878	36.158529	74.994202
271.549093	41.767312	74.999207
271.207697	35.157637	75.004212
270.581425	41.473929	75.009217
270.058369	49.500536	75.014222
269.140823	37.687289	75.019226
268.288967	49.863234	75.024231
268.464445	43.177472	75.029236
268.031972	41.185443	75.034241
266.517380	34.863708	75.039246
266.085558	33.128620	75.044250
265.370801	38.926007	75.049255
264.990948	35.030094	75.054260
263.640783	41.461780	75.059265
262.782505	43.658208	75.064270
262.694936	34.126980	75.069274
262.143954	49.930842	75.074279
261.750361	37.226677	75.079284
260.548541	41.247210	75.084289
259.662311	43.834449	75.089294
259.202075	34.548708	75.094298
258.777686	46.289080	75.099303
258.567440	34.913447	75.104308
257.839839	41.704788	75.109313
256.681031	38.653716	75.114318
256.196639	40.049377	75.119322
255.882585	41.471500	75.124327
254.874656	48.190837	75.129332
253.949961	36.252583	75.134337
253.278372	32.311715	75.139342
253.082444	36.305941	75.144346
252.053605	41.394885	75.149351
251.442050	30.485355	75.154356
250.942916	36.956423	75.159361
250.314824	41.230854	75.164366
249.039759	31.655543	75.169370
248.380253	39.082579	75.174375
248.023097	29.274210	75.179380
247.543160	28.906129	75.184385
247.239382	45.662482	75.189390
246.624362	32.627771	75.194394
245.603098	46.071785	75.199399
245.123046	42.187116	75.204404
244.804185	36.113172	75.209409
243.314081	42.478868	75.214414
243.111718	32.781439	75.219418
242.279784	34.778132	75.224423
241.484074	48.577276	75.229428
240.730178	38.546721	75.234433
239.976800	45.023632	75.239438
239.741086	37.706410	75.244442
239.343687	39.513983	75.249447
238.338999	39.040323	75.254452
237.464722	37.320582	75.259457
236.743344	41.029569	75.264462
236.541081	43.544049	75.269466
235.571929	39.885588	75.274471
234.676139	36.215433	75.279476
234.250156	30.727851	75.284481
233.562973	41.920334	75.289486
233.621057	33.994883	75.294490
232.455285	38.105876	75.299495
231.472538	46.447043	75.304500
231.438452	33.704501	75.309505
230.054992	51.577578	75.314510
229.169722	40.665952	75.319514
228.592239	49.906033	75.324519
228.202668	44.841574	75.329524
227.954132	48.341143	75.334529
227.614891	48.513607	75.339534
226.526601	46.430595	75.344538
225.773088	48.293367	75.349543
225.399535	51.074853	75.354548
224.353855	36.314230	75.359553
223.232746	46.956155	75.364558
222.975024	45.868255	75.369562
222.384676	47.477933	75.374567
222.010072	33.343613	75.379572
221.534284	46.585555	75.384577
220.256000	46.004133	75.389582
219.897694	39.288353	75.394586
219.133386	37.808131	75.399591
218.769395	34.770714	75.404596
217.692961	39.525059	75.409601
217.045300	39.114338	75.414606
216.508007	39.392495	75.419610
215.925772	49.741933	75.424615
215.033967	47.638640	75.429620
214.442767	39.479232	75.434625
213.815479	47.730620	75.439630
213.670387	37.751251	75.444634
212.363950	44.136567	75.449639
211.768595	41.057189	75.454644
211.256901	37.149189	75.459649
210.772652	44.746990	75.464654
209.937529	37.061712	75.469658
209.185703	41.447343	75.474663
208.449755	42.768000	75.479668
208.131154	48.779789	75.484673
207.035344	43.514116	75.489678
206.519112	39.102215	75.494682
205.873593	37.995719	75.499687
205.356498	41.071327	75.504692
205.027049	38.838958	75.509697
203.874414	35.763275	75.514702
203.249544	34.252942	75.519706
202.702510	45.670671	75.524711
202.076607	33.388341	75.529716
200.978275	46.833616	75.534721
199.969596	41.729098	75.539726
199.933132	37.541907	75.544730
199.503575	48.748520	75.549735
198.967063	36.838290	75.554740
198.052415	36.186289	75.559745
196.979224	41.216093	75.564750
196.794831	35.261069	75.569754
196.418147	45.375885	75.574759
194.996004	38.457563	75.579764
194.428552	36.422415	75.584769
193.948610	37.585565	75.589774
193.736454	37.904930	75.594778
193.119498	44.224482	75.599783
192.063574	44.135903	75.604788
191.643528	43.436585	75.609793
190.695536	48.943173	75.614798
189.541605	39.376965	75.619802
189.354553	43.639439	75.624807
188.552597	36.511855	75.629812
188.428050	39.884424	75.634817
187.655227	42.936152	75.639822
186.909525	33.293824	75.644826
186.194139	38.206659	75.649831
185.642604	39.266109	75.654836
184.964091	43.867138	75.659841
184.016324	46.634525	75.664846
183.945100	35.873831	75.669850
183.123401	41.428091	75.674855
181.970966	38.335041	75.679860
181.166272	41.595279	75.684865
180.563760	49.568333	75.689870
180.536796	26.060393	75.694874
179.360820	41.388312	75.699879
178.523734	38.208714	75.704884
178.166985	29.302314	75.709889
177.916581	43.176946	75.714894
177.159429	36.154187	75.719898
175.607219	42.712748	75.724903
175.202259	38.981703	75.729908
174.825822	34.001898	75.734913
174.253862	42.629244	75.739918
174.150146	34.206046	75.744922
172.799372	44.167091	75.749927
172.292875	44.952858	75.754932
171.941526	45.171416	75.759937
170.974402	37.910901	75.764942
169.844168	47.004156	75.769946
168.936136	45.266167	75.774951
168.584034	47.872351	75.779956
168.725751	42.781541	75.784961
167.707568	49.977206	75.789966
166.884435	39.341132	75.794970
166.260361	45.524630	75.799975
165.852472	47.508929	75.804980
165.487982	42.979803	75.809985
164.339747	48.562482	75.814990
163.758515	40.450387	75.819994
162.956236	42.683650	75.824999
162.171137	46.044849	75.830004
161.514017	38.156168	75.835009
160.772912	51.388382	75.840014
160.782482	36.708697	75.845018
160.073737	42.875734	75.850023
158.555546	48.787063	75.855028
158.028519	36.332865	75.860033
157.488207	51.414365	75.865038
157.399669	39.760724	75.870042
156.658158	45.004163	75.875047
155.392488	43.520325	75.880052
154.795154	33.950546	75.885057
154.294857	43.955762	75.890062
154.136553	45.457142	75.895066
153.039087	40.901391	75.900071
152.073438	39.018056	75.905076
151.639550	44.674491	75.910081
151.292883	48.986073	75.915086
150.813968	41.422216	75.920090
150.024123	48.379626	75.925095
148.977163	40.157295	75.930100
148.798928	39.782126	75.935105
147.590259	50.766047	75.940110
146.954160	35.815583	75.945114
146.428052	45.485872	75.950119
145.786002	40.794428	75.955124
145.514482	47.263913	75.960129
144.497583	42.906630	75.965134
143.867829	39.342323	75.970138
143.165024	34.176446	75.975143
142.813607	38.313742	75.980148
141.951073	27.146231	75.985153
140.906134	39.403445	75.990158
140.608989	37.823524	75.995162
140.196944	35.117059	76.000167
139.014881	33.052197	76.005172
138.629693	39.017833	76.010177
137.523693	40.181476	76.015182
137.779719	38.295729	76.020186
136.730519	37.313546	76.025191
135.463624	41.674096	76.030196
135.439187	36.567205	76.035201
134.855479	52.141328	76.040206
133.943374	45.829264	76.045210
132.979742	43.565569	76.050215
132.105897	42.230574	76.055220
132.324981	28.440010	76.060225
131.287059	38.813229	76.065230
130.425853	36.851747	76.070234
129.841207	39.072393	76.075239
129.157705	49.188831	76.080244
128.912301	37.113934	76.085249
128.234078	42.940221	76.090254
127.015543	39.540771	76.095258
126.603401	40.746739	76.100263
126.242817	44.033946	76.105268
125.960095	39.157476	76.110273
124.499853	42.979583	76.115278
124.130263	36.478514	76.120282
123.358342	32.553687	76.125287
122.346915	44.835529	76.130292
121.404122	38.268171	76.135297
120.870626	44.475080	76.140302
120.773258	40.072100	76.145306
120.411333	42.946361	76.150311
119.900818	40.249293	76.155316
119.166163	36.649684	76.160321
118.186274	49.309700	76.165326
117.482213	35.147524	76.170330
116.396653	41.382544	76.175335
115.549429	36.887833	76.180340
115.593271	36.899875	76.185345
115.021013	41.422475	76.190350
114.626643	37.962567	76.195354
113.322769	40.684264	76.200359
112.474046	37.255811	76.205364
112.464696	40.140079	76.210369
111.618187	43.233542	76.215374
110.588444	36.520783	76.220378
110.113484	39.225412	76.225383
109.624786	45.475642	76.230388
109.291021	34.102393	76.235393
108.033543	41.856628	76.240398
107.434338	36.677395	76.245402
106.866002	36.542635	76.250407
106.270587	35.497562	76.255412
105.407091	37.248596	76.260417
104.458502	39.643981	76.265422
104.134727	32.892762	76.270426
103.676367	33.916869	76.275431
102.687077	42.487776	76.280436
102.094497	38.408199	76.285441
100.986736	31.594348	76.290446
101.050771	44.179350	76.295450
100.489478	35.881172	76.300455
99.937692	39.088486	76.305460
99.110381	32.950578	76.310465
97.995027	40.144411	76.315470
97.800942	39.218265	76.320474
97.219884	34.983888	76.325479
96.355426	39.515242	76.330484
96.069502	28.484455	76.335489
95.281459	40.598213	76.340494
94.568967	40.629948	76.345498
93.734473	33.091279	76.350503
92.935825	36.623390	76.355508
92.056642	36.369473	76.360513
91.279678	36.666957	76.365518
90.887117	34.274362	76.370522
90.613350	36.912215	76.375527
89.825898	40.778433	76.380532
88.925688	39.111769	76.385537
87.925257	44.991027	76.390542
87.364364	39.871921	76.395546
87.485529	38.658957	76.400551
86.507697	41.148898	76.405556
85.526251	38.023896	76.410561
84.769765	40.653580	76.415566
84.459779	37.751077	76.420570
84.170857	39.937186	76.425575
82.842695	40.436118	76.430580
82.098838	37.520808	76.435585
81.406192	43.355713	76.440590
81.512043	38.202815	76.445594
80.836500	44.030262	76.450599
80.083769	50.877693	76.455604
79.509716	33.679671	76.460609
78.476395	38.930241	76.465614
77.588493	33.532133	76.470618
77.073861	31.152701	76.475623
76.532407	43.517297	76.480628
76.271309	35.638028	76.485633
74.721241	40.712394	76.490638
74.282997	38.544706	76.495642
73.627699	37.185917	76.500647
73.337006	45.790498	76.505652
72.999906	35.911162	76.510657
71.941993	40.265220	76.515662
71.264894	38.656020	76.520666
70.656510	37.769142	76.525671
69.739420	40.906991	76.530676
68.918678	34.966742	76.535681
68.357096	32.246294	76.540686
67.937269	35.503531	76.545690
67.419951	29.852360	76.550695
66.387158	39.376383	76.555700
65.809915	33.269569	76.560705
65.189553	38.235086	76.565710
64.977736	42.048928	76.570714
63.740518	32.065575	76.575719
63.107486	36.511143	76.580724
62.251699	36.870092	76.585729
61.639113	33.777736	76.590734
61.322472	33.642268	76.595738
61.101514	31.583431	76.600743
59.864745	41.937926	76.605748
59.296333	38.524710	76.610753
58.873415	37.876338	76.615758
58.262517	38.417004	76.620762
57.300568	39.360589	76.625767
56.426870	42.250249	76.630772
56.385843	43.808622	76.635777
55.251758	35.526121	76.640782
54.391270	30.751277	76.645786
53.982845	35.296641	76.650791
53.540564	39.347513	76.655796
53.086647	31.435927	76.660801
51.916848	41.547932	76.665806
51.084115	36.678774	76.670810
50.615029	43.132463	76.675815
49.985098	40.508075	76.680820
49.423713	40.075754	76.685825
48.414320	45.182173	76.690830
48.195991	39.172657	76.695834
47.722232	45.322741	76.700839
46.623366	55.308327	76.705844
46.164309	36.724757	76.710849
45.086995	47.367643	76.715854
45.025341	44.425536	76.720858
44.440323	35.443611	76.725863
43.203304	45.175260	76.730868
42.383542	35.532187	76.735873
41.915416	36.877984	76.740878
41.772301	38.993533	76.745882
41.009874	38.667396	76.750887
40.096629	41.219593	76.755892
39.812877	43.114724	76.760897
39.021497	43.518602	76.765902
37.872915	36.465290	76.770906
37.078703	44.875793	76.775911
36.386958	57.095641	76.780916
36.433820	37.698098	76.785921
35.913602	42.791152	76.790926
35.115710	38.301219	76.795930
34.325292	36.057248	76.800935
33.201051	47.667984	76.805940
33.198465	36.610936	76.810945
32.010110	38.112614	76.815950
31.104165	39.559785	76.820954
30.760103	40.393787	76.825959
30.271043	38.997457	76.830964
29.953821	34.922867	76.835969
28.909865	42.069069	76.840974
28.270441	37.955984	76.845978
28.080592	36.928244	76.850983
26.833897	43.056537	76.855988
26.432678	33.110171	76.860993
25.523207	37.492608	76.865998
24.938842	33.815443	76.871002
24.004160	34.492918	76.876007
22.907865	38.411571	76.881012
22.930296	23.971143	76.886017
22.221838	41.897466	76.891022
21.875859	32.109448	76.896026
21.375861	39.938438	76.901031
20.389717	44.657960	76.906036
20.155463	33.259401	76.911041
19.022434	39.872612	76.916046
18.027439	37.069922	76.921050
17.624531	35.888510	76.926055
16.947339	39.768700	76.931060
16.779555	32.456455	76.936065
16.113611	35.327180	76.941070
14.771684	37.980880	76.946074
14.421046	36.513588	76.951079
13.871289	49.510298	76.956084
12.745212	28.410680	76.961089
11.900389	48.394604	76.966094
11.302681	46.533060	76.971098
11.297297	33.555740	76.976103
10.454424	44.434050	76.981108
10.088566	38.925889	76.986113
8.891780	35.021565	76.991118
8.289172	39.372406	76.996122
8.293829	30.905139	77.001127
7.282400	39.564759	77.006132
6.537610	39.932831	77.011137
5.846634	37.665123	77.016142
5.466781	43.517958	77.021147
4.601956	38.406357	77.026151
3.515363	41.423033	77.031156
3.368765	34.086909	77.036161