Fri Mar 05 19:54:33 2021

Number of Points = 14582

Depth (nm)	Load (N)	Time (s)
-1.701243	87.562623	0.000000
-1.336705	87.838831	0.005005
-1.984165	73.156661	0.010010
-3.869307	15.679680	0.015014
-8.025714	1.101511	0.020019
-13.899359	7.516673	0.025024
-18.706531	5.698848	0.030029
-23.171688	7.291019	0.035034
-27.017197	6.929880	0.040038
-30.499762	-2.135507	0.045043
-34.385412	1.952007	0.050048
-38.020257	4.542430	0.055053
-41.748798	3.829922	0.060058
-45.619985	3.750450	0.065062
-49.000890	4.051666	0.070067
-52.941652	12.361587	0.075072
-56.517231	2.316024	0.080077
-60.392466	-0.837811	0.085082
-64.549837	7.197598	0.090086
-68.003572	3.987575	0.095091
-72.129352	13.798325	0.100096
-75.744516	7.837072	0.105101
-79.842269	0.185065	0.110106
-83.957077	7.477285	0.115110
-87.119345	1.976809	0.120115
-90.949767	7.416500	0.125120
-94.411262	2.219234	0.130125
-97.996416	0.977741	0.135130
-101.996800	0.807007	0.140134
-105.280203	-11.428139	0.145139
-109.475284	2.897452	0.150144
-113.162253	-4.813721	0.155149
-117.016302	-1.853900	0.160154
-121.180434	4.317160	0.165158
-124.501778	2.256187	0.170163
-128.166269	-0.704081	0.175168
-131.874401	-8.817119	0.180173
-135.884518	-0.086009	0.185178
-139.894670	-5.897403	0.190182
-143.334275	5.693146	0.195187
-147.223824	4.657986	0.200192
-150.803148	-2.029524	0.205197
-154.371574	-2.918790	0.210202
-158.503007	-10.046465	0.215206
-162.046219	-14.350655	0.220211
-166.174646	7.571535	0.225216
-170.205403	7.281182	0.230221
-174.050892	9.623145	0.235226
-177.885531	9.236856	0.240230
-180.967830	-5.711066	0.245235
-184.720244	14.881728	0.250240
-188.611379	7.007708	0.255245
-192.248284	1.857501	0.260250
-196.133223	4.625259	0.265254
-199.410581	0.300774	0.270259
-203.679544	5.512576	0.275264
-207.525359	8.586342	0.280269
-211.066877	4.928494	0.285274
-215.123356	7.523385	0.290278
-218.726560	4.104049	0.295283
-222.525962	13.818800	0.300288
-225.795265	9.354293	0.305293
-229.729127	0.362810	0.310298
-233.427603	0.380653	0.315302
-237.417037	0.872286	0.320307
-241.295280	17.646978	0.325312
-245.379968	7.782310	0.330317
-248.375434	11.305473	0.335322
-252.564769	13.913745	0.340326
-255.891853	-3.999069	0.345331
-260.389791	5.179097	0.350336
-263.825788	-2.429965	0.355341
-267.551794	0.145383	0.360346
-271.316935	5.585968	0.365350
-274.718100	-3.930421	0.370355
-278.792988	6.137456	0.375360
-282.760354	1.095328	0.380365
-286.310657	0.268020	0.385370
-290.317288	8.319161	0.390374
-294.121273	4.715947	0.395379
-297.858471	3.402829	0.400384
-301.331826	7.136373	0.405389
-305.071935	8.083479	0.410394
-308.915643	2.586423	0.415398
-312.313947	-4.877196	0.420403
-316.430622	6.309150	0.425408
-320.218224	-3.760490	0.430413
-323.806902	14.500874	0.435418
-327.837638	16.527300	0.440422
-331.543505	7.308785	0.445427
-335.541186	3.875328	0.450432
-339.321372	17.830718	0.455437
-342.635230	-2.044204	0.460442
-346.727864	2.425343	0.465446
-350.347844	0.352436	0.470451
-354.031280	2.367616	0.475456
-357.833556	1.418215	0.480461
-360.910195	3.935771	0.485466
-365.227851	5.990717	0.490470
-369.191771	-2.790723	0.495475
-373.379329	-0.759687	0.500480
-376.827195	4.242479	0.505485
-380.817096	2.167176	0.510490
-384.490615	8.884814	0.515494
-387.819314	0.932382	0.520499
-391.455198	12.377978	0.525504
-395.099141	6.688323	0.530509
-399.115868	1.852968	0.535514
-403.424686	-0.210802	0.540518
-406.514472	-6.883031	0.545523
-410.467177	3.640202	0.550528
-414.214779	3.426473	0.555533
-417.764741	-3.612232	0.560538
-421.912418	-6.827626	0.565542
-425.369041	-17.350466	0.570547
-429.289820	-7.650737	0.575552
-433.310633	2.662635	0.580557
-437.025430	-8.178511	0.585562
-440.609546	-3.078811	0.590566
-444.035242	-10.570970	0.595571
-448.281864	-3.895773	0.600576
-452.420210	-3.815238	0.605581
-455.560496	-3.477759	0.610586
-459.563042	-4.883867	0.615590
-462.841353	-5.218187	0.620595
-466.721280	0.783485	0.625600
-470.899992	-7.111930	0.630605
-474.383928	-3.772265	0.635610
-478.321106	-1.402567	0.640614
-481.913961	-7.147545	0.645619
-485.768230	-4.778460	0.650624
-489.430563	-8.110664	0.655629
-493.136336	-1.964877	0.660634
-497.482287	0.418093	0.665638
-501.125288	-8.374938	0.670643
-505.000142	6.392145	0.675648
-508.364147	2.537668	0.680653
-511.710085	-0.316761	0.685658
-515.771169	-1.297115	0.690662
-519.615654	-3.646139	0.695667
-523.456230	4.214848	0.700672
-527.385990	4.946587	0.705677
-530.919129	5.304331	0.710682
-534.556331	3.868383	0.715686
-537.993428	0.189625	0.720691
-542.140706	4.590955	0.725696
-545.968415	2.551526	0.730701
-549.718259	1.783289	0.735706
-553.226250	5.461220	0.740710
-557.549689	2.537485	0.745715
-560.912836	0.660419	0.750720
-564.934779	4.064071	0.755725
-568.486458	-2.772277	0.760730
-572.540185	-1.180160	0.765734
-575.821444	-5.035138	0.770739
-579.802625	-0.102043	0.775744
-583.918114	3.554699	0.780749
-587.355368	4.537444	0.785754
-591.061007	2.407628	0.790758
-594.434301	-2.421357	0.795763
-597.992334	-0.867379	0.800768
-601.904397	-0.237691	0.805773
-605.823732	0.544550	0.810778
-610.099279	1.320624	0.815782
-613.176712	-1.948706	0.820787
-617.482310	3.007890	0.825792
-621.415714	2.504053	0.830797
-624.993139	0.202424	0.835802
-628.525082	0.296774	0.840806
-632.512584	-8.519854	0.845811
-636.273836	0.724212	0.850816
-640.080924	-5.066716	0.855821
-643.554090	-7.536356	0.860826
-647.522704	1.114814	0.865830
-650.990143	-4.826551	0.870835
-654.991727	-1.075925	0.875840
-659.278044	1.291501	0.880845
-662.658910	-7.782841	0.885850
-666.519980	-4.201300	0.890854
-669.627293	-6.782970	0.895859
-673.846997	6.993954	0.900864
-677.618247	13.571523	0.905869
-681.366461	-2.325821	0.910874
-685.598819	2.992925	0.915878
-689.017896	-3.556919	0.920883
-692.441734	-2.757513	0.925888
-696.360329	8.391485	0.930893
-700.540253	-3.685330	0.935898
-704.687017	2.863968	0.940902
-707.529820	-3.068311	0.945907
-711.855801	0.716897	0.950912
-715.508230	4.258871	0.955917
-718.986099	0.933821	0.960922
-722.621420	0.926561	0.965926
-726.240570	-5.039331	0.970931
-730.309699	2.811184	0.975936
-734.198517	8.575006	0.980941
-737.896755	6.474201	0.985946
-741.886103	4.320576	0.990950
-745.236152	-2.828408	0.995955
-748.856556	1.416538	1.000960
-752.952351	2.943145	1.005965
-756.566045	-2.651417	1.010970
-760.713096	8.270842	1.015974
-763.947062	7.363733	1.020979
-767.938865	6.468933	1.025984
-771.537602	9.485179	1.030989
-774.927355	4.832550	1.035994
-778.755480	11.348399	1.040998
-782.735396	0.487122	1.046003
-786.868866	4.353660	1.051008
-790.508534	2.789196	1.056013
-794.093592	0.735047	1.061018
-798.088918	11.488042	1.066022
-801.761216	1.031790	1.071027
-805.457804	5.481381	1.076032
-809.283623	3.744852	1.081037
-812.816916	1.231457	1.086042
-817.128892	3.822460	1.091046
-820.617814	1.781371	1.096051
-824.606040	5.468643	1.101056
-828.014933	8.651745	1.106061
-831.466555	4.439590	1.111066
-835.883461	4.044931	1.116070
-839.364827	2.349586	1.121075
-843.006313	0.881687	1.126080
-847.020107	2.712311	1.131085
-850.545518	8.191150	1.136090
-854.226217	13.951858	1.141094
-857.984920	3.342355	1.146099
-861.901723	-5.139820	1.151104
-865.915535	2.508113	1.156109
-869.292159	-4.811474	1.161114
-873.187947	-1.753901	1.166118
-877.068525	0.478094	1.171123
-880.427100	2.990916	1.176128
-884.465132	5.352171	1.181133
-888.303204	-4.878739	1.186138
-892.314223	2.229483	1.191142
-895.765459	-7.303175	1.196147
-899.154117	-3.771556	1.201152
-903.224302	7.794647	1.206157
-907.131469	0.266625	1.211162
-911.197067	0.367868	1.216166
-914.708150	0.262196	1.221171
-918.213082	-6.570034	1.226176
-922.066262	2.720694	1.231181
-925.753332	4.092369	1.236186
-929.562567	7.118851	1.241190
-933.255792	5.900634	1.246195
-936.790728	1.233613	1.251200
-940.920739	7.334364	1.256205
-944.250669	11.804392	1.261210
-948.643715	8.042550	1.266214
-952.081246	4.515864	1.271219
-955.928924	4.558687	1.276224
-959.923567	8.401748	1.281229
-963.526367	3.658889	1.286234
-967.366868	5.583430	1.291238
-970.993075	9.701906	1.296243
-974.550332	-1.171411	1.301248
-978.551969	11.700686	1.306253
-982.113870	-6.501414	1.311258
-986.264506	6.139054	1.316262
-989.810351	5.534438	1.321267
-993.305567	4.218423	1.326272
-996.927037	8.386641	1.331277
-1001.039915	-1.204052	1.336282
-1005.108390	13.877006	1.341286
-1008.623535	5.466468	1.346291
-1012.463910	3.130217	1.351296
-1016.377873	-0.067874	1.356301
-1019.749588	-0.265061	1.361306
-1023.703385	7.080226	1.366310
-1027.810154	7.885255	1.371315
-1031.307081	10.732648	1.376320
-1035.155681	13.328787	1.381325
-1038.474514	-0.203403	1.386330
-1042.550779	5.242386	1.391334
-1046.104536	-1.804182	1.396339
-1049.831736	9.518174	1.401344
-1053.823360	2.213645	1.406349
-1057.428382	-0.051364	1.411354
-1061.408477	2.436540	1.416358
-1065.066438	14.679809	1.421363
-1069.090562	18.213961	1.426368
-1072.549873	9.791439	1.431373
-1076.059758	4.781590	1.436378
-1079.885521	1.713000	1.441382
-1083.682489	-4.466723	1.446387
-1087.545455	1.501677	1.451392
-1091.629605	9.038232	1.456397
-1095.253849	-2.825517	1.461402
-1099.145765	8.419181	1.466406
-1102.161811	-1.744149	1.471411
-1106.148249	0.241806	1.476416
-1110.158772	13.241686	1.481421
-1114.230759	3.444391	1.486426
-1118.124860	11.541935	1.491430
-1121.435585	1.222345	1.496435
-1125.057603	-0.506840	1.501440
-1129.039501	4.239616	1.506445
-1132.544339	3.716965	1.511450
-1136.271908	15.745972	1.516454
-1140.158099	15.322183	1.521459
-1143.970132	0.473481	1.526464
-1148.134820	-2.862467	1.531469
-1151.653373	-11.135028	1.536474
-1155.656825	10.421729	1.541478
-1158.959937	1.045554	1.546483
-1162.572151	6.849384	1.551488
-1166.325708	8.269917	1.556493
-1170.200294	-1.017968	1.561498
-1174.015137	-4.133877	1.566502
-1177.919297	1.202605	1.571507
-1181.679145	6.733622	1.576512
-1185.867264	13.895893	1.581517
-1189.198145	-2.300701	1.586522
-1192.771380	1.934208	1.591526
-1196.510790	4.035332	1.596531
-1200.420722	8.169586	1.601536
-1204.321183	6.685344	1.606541
-1208.080622	10.335073	1.611546
-1212.031704	11.405668	1.616550
-1215.310520	1.634615	1.621555
-1218.966402	2.751028	1.626560
-1223.138825	1.425449	1.631565
-1226.812283	-2.238108	1.636570
-1230.686319	7.535820	1.641574
-1234.256567	5.347525	1.646579
-1237.890574	-0.211476	1.651584
-1242.003550	11.899853	1.656589
-1245.431579	3.500987	1.661594
-1249.408335	9.826894	1.666598
-1253.238523	7.927798	1.671603
-1257.179444	0.617100	1.676608
-1260.685958	-0.561086	1.681613
-1264.339210	-5.110889	1.686618
-1268.102515	-3.896787	1.691622
-1271.943617	1.831871	1.696627
-1275.593400	2.283513	1.701632
-1279.565238	8.692259	1.706637
-1283.107479	-2.107260	1.711642
-1286.592327	2.813797	1.716646
-1290.361300	3.853804	1.721651
-1294.336791	6.734016	1.726656
-1298.496449	15.456231	1.731661
-1302.033640	1.470557	1.736666
-1305.872373	3.947287	1.741670
-1309.499322	5.455017	1.746675
-1313.006758	9.091387	1.751680
-1316.997629	2.184595	1.756685
-1320.815947	1.262980	1.761690
-1324.917500	12.342891	1.766694
-1328.196684	3.904563	1.771699
-1331.736334	16.868855	1.776704
-1335.925553	6.355891	1.781709
-1339.681608	-7.511103	1.786714
-1343.672383	6.236591	1.791718
-1347.052271	9.597136	1.796723
-1350.778443	10.734467	1.801728
-1354.833821	10.659810	1.806733
-1358.256082	6.699220	1.811738
-1362.232146	13.682777	1.816742
-1365.775249	4.045717	1.821747
-1369.581459	2.871515	1.826752
-1373.688696	4.222840	1.831757
-1377.156127	1.173084	1.836762
-1381.012398	5.628621	1.841766
-1384.915625	-0.309658	1.846771
-1388.450275	1.386842	1.851776
-1392.456434	11.503866	1.856781
-1395.827032	-0.890398	1.861786
-1399.636524	10.380996	1.866790
-1403.494909	11.763498	1.871795
-1407.130506	11.110812	1.876800
-1411.307291	9.945541	1.881805
-1414.688622	7.262095	1.886810
-1418.568707	5.642495	1.891814
-1422.383559	6.567061	1.896819
-1425.973175	7.789882	1.901824
-1429.884097	7.089849	1.906829
-1433.362342	-0.393952	1.911834
-1437.609303	3.679534	1.916838
-1441.076811	0.976810	1.921843
-1444.815049	3.883945	1.926848
-1448.918570	3.322010	1.931853
-1452.163090	5.768498	1.936858
-1455.895944	8.331022	1.941862
-1459.983920	4.265867	1.946867
-1463.670565	5.425435	1.951872
-1467.582122	11.121536	1.956877
-1471.147493	0.721836	1.961882
-1475.134907	9.577615	1.966886
-1478.873770	14.965394	1.971891
-1482.546936	3.854436	1.976896
-1486.639736	20.600649	1.981901
-1490.296477	-1.649098	1.986906
-1493.911486	3.211102	1.991910
-1497.712584	6.257694	1.996915
-1501.295323	10.056799	2.006912
-1502.454454	6.446724	2.016909
-1499.774119	2.807635	2.026906
-1496.819139	4.068212	2.036902
-1495.011938	4.563641	2.046899
-1493.099725	4.609627	2.056896
-1491.280411	0.255794	2.066893
-1489.127679	10.565813	2.076890
-1487.511630	9.220818	2.086886
-1485.510848	5.810554	2.096883
-1483.388364	7.190238	2.106880
-1481.758561	2.202024	2.116877
-1479.666661	2.426091	2.126874
-1477.576344	5.100919	2.136870
-1475.441225	5.845434	2.146867
-1473.850512	11.426552	2.156864
-1472.223690	9.921949	2.166861
-1470.507292	4.528301	2.176858
-1468.424059	5.964809	2.186854
-1466.299148	4.104147	2.196851
-1464.873833	4.172853	2.206848
-1462.955675	8.111564	2.216845
-1460.731106	6.733895	2.226842
-1458.861177	13.053471	2.236838
-1457.215420	8.784290	2.246835
-1455.262887	12.079617	2.256832
-1453.243229	6.477954	2.266829
-1451.197322	8.755710	2.276826
-1449.373933	5.247563	2.286822
-1447.603573	13.773073	2.296819
-1445.831942	11.864780	2.306816
-1444.071696	11.377775	2.316813
-1442.220517	8.643598	2.326810
-1440.142660	10.390464	2.336806
-1438.320279	13.534539	2.346803
-1436.110078	8.952376	2.356800
-1434.411945	13.668439	2.366797
-1432.710948	17.741419	2.376794
-1430.771238	14.184662	2.386790
-1428.957071	14.110611	2.396787
-1426.970857	15.872162	2.406784
-1424.941838	12.643740	2.416781
-1423.010083	13.997174	2.426778
-1421.068355	12.492718	2.436774
-1419.773524	8.376058	2.446771
-1417.983376	14.411603	2.456768
-1415.604022	9.248172	2.466765
-1413.784066	11.721608	2.476762
-1411.692780	17.031588	2.486758
-1409.928674	7.755635	2.496755
-1408.083426	6.220846	2.506752
-1406.310386	9.126531	2.516749
-1404.414836	3.495830	2.526746
-1402.634386	3.799826	2.536742
-1400.596368	5.846787	2.546739
-1398.501627	6.253630	2.556736
-1396.905066	4.452347	2.566733
-1395.250557	6.464391	2.576730
-1393.396791	5.780876	2.586726
-1391.241743	7.802796	2.596723
-1389.205789	5.928023	2.606720
-1387.549786	5.830376	2.616717
-1385.562594	8.319694	2.626714
-1383.747623	-0.534909	2.636710
-1381.698285	8.026523	2.646707
-1379.989921	11.788893	2.656704
-1378.174909	4.214802	2.666701
-1376.256244	5.725105	2.676698
-1374.191075	7.584588	2.686694
-1372.747725	7.554148	2.696691
-1370.768481	5.341103	2.706688
-1368.393432	4.384694	2.716685
-1366.792721	6.642210	2.726682
-1364.941183	8.747475	2.736678
-1363.146704	11.847131	2.746675
-1361.223316	7.768836	2.756672
-1359.286798	5.829479	2.766669
-1357.324527	10.108589	2.776666
-1355.648337	6.930387	2.786662
-1353.653899	7.754375	2.796659
-1351.885121	9.727635	2.806656
-1349.910505	7.692189	2.816653
-1348.039273	8.428535	2.826650
-1346.183210	7.758900	2.836646
-1344.286844	8.366490	2.846643
-1342.571403	4.618335	2.856640
-1340.376498	6.204454	2.866637
-1338.639773	4.492880	2.876634
-1336.754479	11.053260	2.886630
-1334.918323	11.476286	2.896627
-1332.854385	8.896035	2.906624
-1331.561525	4.247635	2.916621
-1329.202509	3.042780	2.926618
-1327.191268	12.027205	2.936614
-1325.415710	3.068422	2.946611
-1323.857668	7.268575	2.956608
-1321.755027	0.079540	2.966605
-1319.782781	10.901778	2.976602
-1318.616335	9.826223	2.986598
-1316.196413	5.902179	2.996595
-1313.825172	7.381154	3.006592
-1312.351819	6.927533	3.016589
-1310.467098	10.063314	3.026586
-1308.692499	7.799389	3.036582
-1306.675133	10.443421	3.046579
-1304.652060	10.599716	3.056576
-1302.854057	5.992065	3.066573
-1301.350963	3.440020	3.076570
-1299.328981	11.488022	3.086566
-1297.432655	8.333050	3.096563
-1296.113380	9.426192	3.106560
-1293.783995	7.679803	3.116557
-1291.762466	5.599003	3.126554
-1289.774447	10.342997	3.136550
-1287.942971	14.000474	3.146547
-1286.082738	10.794445	3.156544
-1284.018132	9.628856	3.166541
-1282.353666	9.796771	3.176538
-1280.613601	11.564683	3.186534
-1278.857386	15.788420	3.196531
-1276.630323	6.994254	3.206528
-1274.826758	11.673044	3.216525
-1273.081985	12.576530	3.226522
-1271.213280	11.530722	3.236518
-1269.209809	11.687028	3.246515
-1267.439383	14.176404	3.256512
-1265.136486	10.577450	3.266509
-1263.561311	8.282313	3.276506
-1261.730876	14.092071	3.286502
-1259.770623	12.725309	3.296499
-1257.725469	9.898655	3.306496
-1256.051451	9.564537	3.316493
-1254.252727	11.019927	3.326490
-1252.545635	13.209977	3.336486
-1250.661019	6.853250	3.346483
-1248.638044	8.512759	3.356480
-1246.559454	6.643917	3.366477
-1244.900098	11.631595	3.376474
-1242.924716	14.632929	3.386470
-1241.136472	12.687394	3.396467
-1239.161708	9.377812	3.406464
-1237.053828	13.493205	3.416461
-1235.536362	9.909432	3.426458
-1233.297787	5.608701	3.436454
-1231.668962	11.880215	3.446451
-1230.066562	5.644450	3.456448
-1227.813269	10.980787	3.466445
-1226.108918	9.302897	3.476442
-1224.390016	12.514231	3.486438
-1222.075075	15.083885	3.496435
-1220.090183	9.104290	3.506432
-1218.162096	7.311660	3.516429
-1216.915409	7.135943	3.526426
-1214.663334	12.226175	3.536422
-1212.807570	6.410932	3.546419
-1211.059581	7.402371	3.556416
-1209.334409	13.652171	3.566413
-1207.161539	5.654628	3.576410
-1205.336958	6.895920	3.586406
-1203.457470	13.035772	3.596403
-1201.936341	5.733033	3.606400
-1200.236553	6.602719	3.616397
-1198.114570	6.230127	3.626394
-1196.041202	7.411096	3.636390
-1194.255352	7.648074	3.646387
-1191.949610	1.748222	3.656384
-1190.171387	8.734807	3.666381
-1188.594295	12.281488	3.676378
-1186.853135	7.000912	3.686374
-1184.849805	11.834131	3.696371
-1182.835957	5.673093	3.706368
-1180.911271	13.558356	3.716365
-1179.093526	0.039262	3.726362
-1177.273041	6.873833	3.736358
-1175.706792	13.635399	3.746355
-1173.438029	9.227261	3.756352
-1171.640583	4.607162	3.766349
-1169.685489	5.822866	3.776346
-1167.850166	8.728251	3.786342
-1165.999983	8.732328	3.796339
-1164.196467	7.307036	3.806336
-1162.155340	3.124800	3.816333
-1160.245424	3.280377	3.826330
-1158.292810	1.177557	3.836326
-1156.796986	3.668318	3.846323
-1154.819679	-1.512643	3.856320
-1152.476911	-0.033682	3.866317
-1150.765788	-1.878390	3.876314
-1149.565684	1.011786	3.886310
-1147.642403	-2.891059	3.896307
-1145.203321	8.243505	3.906304
-1143.382386	-0.774519	3.916301
-1141.569470	-1.274459	3.926298
-1139.859937	-5.381523	3.936294
-1137.685830	6.117539	3.946291
-1135.898005	0.930588	3.956288
-1134.180400	-0.608831	3.966285
-1132.087759	4.764355	3.976282
-1130.441258	-1.541558	3.986278
-1128.554211	0.945059	3.996275
-1126.501709	2.418374	4.006272
-1124.615732	-3.175845	4.016269
-1123.080974	-0.337608	4.026266
-1121.323903	-1.449123	4.036262
-1118.980134	-0.554496	4.046259
-1117.014107	1.229501	4.056256
-1115.263707	0.561161	4.066253
-1113.270256	-1.180261	4.076250
-1111.507740	-0.546332	4.086246
-1109.816135	-5.029453	4.096243
-1107.934265	2.090617	4.106240
-1105.795652	-1.565588	4.116237
-1103.770969	3.447444	4.126234
-1102.365730	3.405900	4.136230
-1100.368703	-2.225012	4.146227
-1098.546243	-1.570661	4.156224
-1096.636253	-0.083998	4.166221
-1094.492474	-6.385743	4.176218
-1092.904886	-3.481726	4.186214
-1091.062467	5.037296	4.196211
-1089.043044	1.237539	4.206208
-1086.944477	4.876143	4.216205
-1085.377336	2.179778	4.226202
-1083.551164	-0.018019	4.236198
-1081.460316	3.211300	4.246195
-1079.606644	1.053318	4.256192
-1077.870120	2.599321	4.266189
-1075.734038	-2.581709	4.276186
-1074.060608	-0.845613	4.286182
-1072.285559	1.207387	4.296179
-1070.387905	-0.056047	4.306176
-1068.446556	-1.372259	4.316173
-1066.620366	-0.783216	4.326170
-1064.526895	1.340441	4.336166
-1062.876846	-4.125999	4.346163
-1060.828686	-3.043508	4.356160
-1059.087552	4.148063	4.366157
-1057.346315	1.425451	4.376154
-1055.253595	3.692921	4.386150
-1053.228016	1.218519	4.396147
-1051.428487	-0.321312	4.406144
-1049.406105	-1.535204	4.416141
-1048.050245	-6.667216	4.426138
-1046.126656	-6.275313	4.436134
-1043.940957	-5.014279	4.446131
-1041.987575	-4.361875	4.456128
-1040.288201	-10.652499	4.466125
-1038.479290	-6.539635	4.476122
-1036.571654	-5.024125	4.486118
-1034.858080	-9.455445	4.496115
-1032.692407	-3.277536	4.506112
-1030.713965	-7.269636	4.516109
-1028.939875	-10.199584	4.526106
-1027.412957	0.138360	4.536102
-1025.311823	-3.477044	4.546099
-1023.201689	-3.531795	4.556096
-1021.423080	-10.701916	4.566093
-1020.098424	0.048905	4.576090
-1017.478480	-4.399457	4.586086
-1015.932672	-4.105009	4.596083
-1013.764437	-2.547470	4.606080
-1011.434887	-5.289919	4.616077
-1009.995858	-7.223645	4.626074
-1008.561794	-1.609239	4.636070
-1006.546013	-0.368364	4.646067
-1004.677722	3.911876	4.656064
-1002.594282	-4.176978	4.666061
-1000.895133	-5.662824	4.676058
-998.932657	-5.543941	4.686054
-997.013184	-0.247147	4.696051
-995.041139	-3.511884	4.706048
-993.653620	-6.744727	4.716045
-991.611116	-7.663367	4.726042
-989.554788	-1.303719	4.736038
-987.739104	-2.691348	4.746035
-986.005680	-9.258960	4.756032
-984.065777	-2.770164	4.766029
-981.936387	-1.569540	4.776026
-980.157952	-0.260690	4.786022
-978.464496	-0.021405	4.796019
-976.651449	2.824539	4.806016
-974.379594	-3.366532	4.816013
-972.720295	-5.166511	4.826010
-971.066530	-2.224041	4.836006
-968.933118	3.011728	4.846003
-967.113812	-0.970667	4.856000
-965.329009	2.028223	4.865997
-963.150792	-2.891028	4.875994
-961.426195	-1.707766	4.885990
-959.758125	5.511360	4.895987
-957.711204	1.167315	4.905984
-955.920507	-0.888924	4.915981
-954.179095	-0.529395	4.925978
-951.899362	4.000893	4.935974
-949.793240	-1.623660	4.945971
-948.180015	3.145830	4.955968
-946.690036	-7.513346	4.965965
-944.591553	-7.561426	4.975962
-943.132773	-7.649329	4.985958
-941.292104	0.669577	4.995955
-938.950462	-7.373666	5.005952
-937.301157	-8.043079	5.015949
-934.810534	-0.273346	5.025946
-932.749857	-2.799048	5.035942
-931.662345	2.210821	5.045939
-929.907088	-0.750783	5.055936
-927.886077	-6.788022	5.065933
-925.628234	-6.378407	5.075930
-923.917273	-5.833988	5.085926
-922.067979	-8.940093	5.095923
-920.166177	-3.315145	5.105920
-918.324145	-3.915884	5.115917
-916.400813	-3.861726	5.125914
-914.543415	-1.922820	5.135910
-912.795930	-3.787383	5.145907
-910.935217	-15.372644	5.155904
-908.862028	-3.179847	5.165901
-907.055741	-5.764330	5.175898
-905.265769	-4.428847	5.185894
-903.215186	-5.653439	5.195891
-901.265935	-4.076575	5.205888
-899.516828	-11.802421	5.215885
-897.801976	-9.272295	5.225882
-895.687334	-15.433421	5.235878
-893.697636	-13.668808	5.245875
-892.003100	-12.114375	5.255872
-890.270513	-8.106031	5.265869
-888.480344	-16.523692	5.275866
-886.621312	-10.320304	5.285862
-884.552461	-9.349913	5.295859
-882.596079	-13.243630	5.305856
-880.439426	-10.343593	5.315853
-878.993618	-10.517804	5.325850
-877.075994	-9.509021	5.335846
-875.119245	-3.978081	5.345843
-873.132875	0.856550	5.355840
-871.261242	-6.790972	5.365837
-869.634117	-5.647323	5.375834
-867.915469	0.318002	5.385830
-866.008152	-3.651546	5.395827
-863.771131	-1.931178	5.405824
-861.916044	-6.375529	5.415821
-860.094275	-8.122454	5.425818
-858.246460	-5.147763	5.435814
-856.429209	-4.876074	5.445811
-854.498722	-15.488770	5.455808
-852.687126	-7.795142	5.465805
-850.734770	-12.215558	5.475802
-848.884952	-3.489089	5.485798
-847.074683	-4.702062	5.495795
-844.997399	-6.961923	5.505792
-842.996859	-8.175307	5.515789
-841.246402	-11.848182	5.525786
-839.631135	-8.108413	5.535782
-837.889913	-8.756133	5.545779
-835.966969	-7.522377	5.555776
-833.831981	-6.181986	5.565773
-831.787721	-5.918141	5.575770
-830.025338	-11.484489	5.585766
-828.473472	-5.914056	5.595763
-826.481799	-11.703366	5.605760
-824.406708	-4.006039	5.615757
-822.340913	-1.800369	5.625754
-820.651932	-2.673410	5.635750
-818.855642	-11.545164	5.645747
-816.946568	-8.493390	5.655744
-815.097740	-3.663566	5.665741
-813.508965	-8.355842	5.675738
-811.474739	-5.894064	5.685734
-809.560665	-5.345709	5.695731
-807.433951	-6.756072	5.705728
-805.527190	-7.303910	5.715725
-803.912246	-3.622483	5.725722
-801.900795	-11.816510	5.735718
-800.018586	-2.030966	5.745715
-798.484878	-3.979700	5.755712
-796.295106	-4.961184	5.765709
-794.335164	0.043530	5.775706
-792.514523	-5.911052	5.785702
-790.744403	0.919264	5.795699
-788.838286	-1.960561	5.805696
-786.969044	-10.273954	5.815693
-785.097860	-10.446618	5.825690
-783.094876	-7.823507	5.835686
-781.648207	-11.332526	5.845683
-779.506627	-10.031034	5.855680
-777.480939	-14.682586	5.865677
-775.837230	-2.518909	5.875674
-773.842890	-7.441765	5.885670
-772.172085	-9.267129	5.895667
-769.719416	-10.320603	5.905664
-767.857068	-10.226578	5.915661
-766.394181	-12.280814	5.925658
-764.502277	-15.172557	5.935654
-762.661555	-5.512983	5.945651
-760.787940	-11.291270	5.955648
-759.009449	-9.121735	5.965645
-756.858708	-5.178532	5.975642
-755.043197	-6.247010	5.985638
-753.364327	-2.741551	5.995635
-751.071932	-2.192027	6.005632
-749.412951	-2.837593	6.015629
-747.556487	-9.341024	6.025626
-745.965887	-5.725139	6.035622
-743.863534	-4.234187	6.045619
-741.672323	-8.452690	6.055616
-740.003379	-8.056158	6.065613
-738.175416	-5.539249	6.075610
-736.213417	-3.544283	6.085606
-734.326220	-7.227883	6.095603
-732.759572	-0.216584	6.105600
-730.563070	-1.120136	6.115597
-728.892478	-12.823320	6.125594
-726.913790	-10.123647	6.135590
-724.999985	0.091128	6.145587
-723.273606	-7.646763	6.155584
-721.105690	-10.413631	6.165581
-719.377337	-5.106583	6.175578
-717.713078	-4.543497	6.185574
-715.491248	-0.469507	6.195571
-713.808183	-0.087844	6.205568
-711.691152	-1.632364	6.215565
-710.140516	-6.774798	6.225562
-708.248248	3.301331	6.235558
-706.509815	-5.175845	6.245555
-704.471133	-4.462577	6.255552
-702.051743	-2.264351	6.265549
-700.646366	2.909585	6.275546
-699.061590	-10.788292	6.285542
-696.878211	-8.133930	6.295539
-695.066920	0.919358	6.305536
-693.082876	6.109788	6.315533
-691.137270	-2.859956	6.325530
-689.494881	5.604539	6.335526
-687.425903	0.110875	6.345523
-685.580452	-5.555491	6.355520
-683.648243	3.487963	6.365517
-681.858441	-1.280563	6.375514
-680.255434	0.722862	6.385510
-678.198275	2.307937	6.395507
-676.085130	-2.292773	6.405504
-674.127969	5.999863	6.415501
-672.588648	3.941363	6.425498
-670.846147	2.301981	6.435494
-668.822362	4.328186	6.445491
-666.800310	0.433617	6.455488
-664.953343	0.280706	6.465485
-663.113761	-2.151022	6.475482
-661.280594	0.262486	6.485478
-659.724273	-5.215563	6.495475
-657.523652	-5.576549	6.505472
-655.155034	-3.728583	6.515469
-654.013998	-8.715542	6.525466
-652.026727	-6.236648	6.535462
-650.087036	-7.771729	6.545459
-648.029398	-1.276178	6.555456
-646.273300	-5.824556	6.565453
-644.297946	-1.077961	6.575450
-642.366801	-6.686934	6.585446
-640.539314	-5.050924	6.595443
-638.893453	-2.103790	6.605440
-636.835563	-6.776165	6.615437
-634.816368	-4.363934	6.625434
-633.132398	1.142906	6.635430
-631.344142	-1.460599	6.645427
-629.391829	2.915481	6.655424
-627.298673	2.773797	6.665421
-625.844207	3.591516	6.675418
-623.868708	1.217050	6.685414
-621.625917	1.763572	6.695411
-620.268994	5.503722	6.705408
-618.098400	2.507567	6.715405
-615.970858	3.369348	6.725402
-614.509502	9.909665	6.735398
-612.257197	3.657300	6.745395
-610.376339	11.071659	6.755392
-608.821299	9.683320	6.765389
-606.689587	4.456015	6.775386
-605.139364	10.431089	6.785382
-603.137581	9.254021	6.795379
-601.072251	11.365229	6.805376
-599.507795	6.935914	6.815373
-597.495056	11.408162	6.825370
-595.587680	3.541961	6.835366
-593.474454	3.303942	6.845363
-591.818131	9.731025	6.855360
-589.843938	5.201528	6.865357
-588.218740	9.705689	6.875354
-586.402697	5.256720	6.885350
-584.159008	6.647873	6.895347
-582.416875	9.813357	6.905344
-580.226166	5.558757	6.915341
-578.791397	7.521232	6.925338
-576.969808	7.156128	6.935334
-574.882987	5.599184	6.945331
-573.249432	5.096749	6.955328
-571.483908	4.996394	6.965325
-569.291629	6.015246	6.975322
-567.117350	2.405915	6.985318
-565.586397	3.880929	6.995315
-563.678277	1.736748	7.005312
-561.457680	0.606870	7.015309
-560.112808	3.891086	7.025306
-558.091996	6.884180	7.035302
-556.131203	11.137393	7.045299
-554.462988	8.870484	7.055296
-552.419988	5.419502	7.065293
-550.396484	-1.629947	7.075290
-548.540820	4.747959	7.085286
-547.035089	9.119651	7.095283
-545.167698	5.177249	7.105280
-543.133657	11.832989	7.115277
-541.214206	13.915446	7.125274
-539.146548	6.607896	7.135270
-537.472754	6.050111	7.145267
-535.230581	6.094707	7.155264
-533.932187	15.054798	7.165261
-531.863774	8.007660	7.175258
-530.035574	4.763108	7.185254
-527.931206	-1.347132	7.195251
-525.978952	-0.681485	7.205248
-524.198854	-0.995712	7.215245
-522.286362	2.215240	7.225242
-520.532122	1.813567	7.235238
-519.012140	-2.622805	7.245235
-517.016710	2.905436	7.255232
-514.826745	1.437860	7.265229
-512.799684	-0.287907	7.275226
-511.123654	3.653978	7.285222
-509.182749	-0.236979	7.295219
-507.177284	6.300197	7.305216
-505.483346	4.122372	7.315213
-503.638205	1.588821	7.325210
-501.987963	4.203776	7.335206
-499.942980	2.677262	7.345203
-497.935624	1.646234	7.355200
-495.952364	1.509584	7.365197
-494.155177	0.513701	7.375194
-492.637143	4.411358	7.385190
-490.595271	9.049575	7.395187
-488.640295	2.745327	7.405184
-486.904346	-2.466043	7.415181
-484.426956	0.372097	7.425178
-483.038608	2.934152	7.435174
-481.229519	1.391640	7.445171
-479.295941	-0.567067	7.455168
-477.352908	-0.820436	7.465165
-475.598869	-0.006252	7.475162
-473.801218	-1.281668	7.485158
-471.276549	2.861045	7.495155
-469.802480	2.437833	7.505152
-467.908730	2.042341	7.515149
-466.030219	2.637708	7.525146
-464.475274	6.452121	7.535142
-462.507359	-0.417858	7.545139
-460.309663	3.769185	7.555136
-458.426166	3.125864	7.565133
-456.757833	6.254280	7.575130
-454.633299	9.502484	7.585126
-452.981448	8.154049	7.595123
-451.318740	5.149139	7.605120
-449.594162	5.614362	7.615117
-447.124547	-4.533093	7.625114
-445.244899	2.171071	7.635110
-443.601990	4.709871	7.645107
-441.738002	3.234412	7.655104
-439.911062	1.340132	7.665101
-438.141717	3.096113	7.675098
-436.187768	-0.470028	7.685094
-434.131294	7.982235	7.695091
-432.171697	4.560458	7.705088
-430.409788	7.896585	7.715085
-428.492053	5.240972	7.725082
-426.741853	10.399504	7.735078
-425.016658	10.417802	7.745075
-423.015234	4.115660	7.755072
-420.820497	6.405314	7.765069
-419.279853	9.323619	7.775066
-417.199419	11.405737	7.785062
-415.568925	8.677574	7.795059
-413.598238	8.558789	7.805056
-411.886900	10.145631	7.815053
-410.026949	15.466656	7.825050
-407.902852	5.758083	7.835046
-405.912629	11.898313	7.845043
-404.167743	7.107149	7.855040
-402.268789	3.950868	7.865037
-400.471688	9.951409	7.875034
-398.477151	9.726197	7.885030
-396.743690	6.397394	7.895027
-394.818331	7.699025	7.905024
-392.852989	1.382141	7.915021
-390.850920	-1.465329	7.925018
-389.199189	7.196859	7.935014
-387.276177	3.607273	7.945011
-385.607411	4.989351	7.955008
-383.625154	6.480855	7.965005
-381.668167	4.460065	7.975002
-379.658590	4.033520	7.984998
-377.967498	-1.189564	7.994995
-376.125274	-2.743603	8.004992
-374.421387	-1.436600	8.014989
-372.099496	3.899126	8.024986
-370.568362	4.859501	8.034982
-368.639185	12.034251	8.044979
-366.260795	7.006186	8.054976
-364.741883	5.660086	8.064973
-363.280681	3.154774	8.074970
-360.941148	9.139805	8.084966
-359.107227	6.985521	8.094963
-357.454060	1.766925	8.104960
-355.389556	2.384793	8.114957
-353.537625	1.373959	8.124954
-351.648878	-1.215387	8.134950
-349.759192	8.356217	8.144947
-347.872022	9.469771	8.154944
-345.894915	-1.303184	8.164941
-344.169991	-0.500044	8.174938
-342.369299	4.956809	8.184934
-340.413544	4.499414	8.194931
-338.303089	1.149945	8.204928
-336.643033	-0.569196	8.214925
-334.616372	-4.911078	8.224922
-332.816279	-4.505194	8.234918
-331.218713	-0.084860	8.244915
-329.519644	2.014001	8.254912
-327.232709	-7.436283	8.264909
-325.254050	-1.625720	8.274906
-323.562319	-0.604109	8.284902
-321.718125	0.933169	8.294899
-319.733604	1.682257	8.304896
-317.873512	-1.085649	8.314893
-315.920800	2.385898	8.324890
-314.224259	6.150971	8.334886
-312.321393	3.955718	8.344883
-310.255071	6.583343	8.354880
-308.331726	5.463249	8.364877
-306.548245	4.490219	8.374874
-304.764399	1.769230	8.384870
-303.237242	1.318698	8.394867
-301.170195	6.756755	8.404864
-298.802260	-0.295374	8.414861
-297.109207	1.700260	8.424858
-295.523702	2.880953	8.434854
-293.448259	1.940279	8.444851
-291.610761	1.943906	8.454848
-289.569115	1.807581	8.464845
-287.987506	0.407310	8.474842
-286.085301	4.712738	8.484838
-283.965874	2.631362	8.494835
-282.444550	-7.091423	8.504832
-280.445499	3.328051	8.514829
-278.142155	-1.372160	8.524826
-276.831177	-2.686596	8.534822
-275.000416	-0.747663	8.544819
-272.758482	-0.945941	8.554816
-270.887406	0.353401	8.564813
-269.114394	-1.238459	8.574810
-266.974108	-4.947893	8.584807
-265.318884	0.780134	8.594803
-263.467208	-4.091134	8.604800
-261.579628	-4.194952	8.614797
-259.672347	-4.540334	8.624794
-257.761391	-4.253141	8.634791
-255.999512	-3.493731	8.644787
-254.222617	-5.738308	8.654784
-252.026274	-1.621904	8.664781
-250.160148	-12.089701	8.674778
-248.304038	-8.575840	8.684775
-246.370431	-5.399609	8.694771
-244.881435	-2.450840	8.704768
-242.779562	-7.736235	8.714765
-240.970775	-6.287981	8.724762
-239.210168	-4.494140	8.734759
-236.904989	-1.031409	8.744755
-235.324579	-4.589885	8.754752
-233.447534	-5.372529	8.764749
-231.677382	-9.264442	8.774746
-229.640359	-2.228367	8.784743
-227.649562	-8.894977	8.794739
-226.221485	-6.973848	8.804736
-223.743396	-12.546634	8.814733
-222.323002	-14.939559	8.824730
-220.398555	-10.863421	8.834727
-218.685384	-10.719898	8.844723
-216.533732	-13.166358	8.854720
-214.681133	-15.940884	8.864717
-212.795127	-13.837035	8.874714
-210.978317	-15.298472	8.884711
-208.941305	-21.318751	8.894707
-207.129745	-8.582972	8.904704
-205.135296	-11.643813	8.914701
-203.295964	-15.027269	8.924698
-201.823709	-13.092650	8.934695
-199.638187	-12.214485	8.944691
-197.777254	-13.701902	8.954688
-195.758151	-5.838724	8.964685
-194.153806	-10.409945	8.974682
-192.631923	-13.262735	8.984679
-190.375288	-4.043237	8.994675
-188.252237	-8.064065	9.004672
-186.547513	-14.214464	9.014669
-184.609584	-5.127264	9.024666
-182.711001	-7.872789	9.034663
-181.012595	-4.343182	9.044659
-178.988578	-9.701364	9.054656
-177.124149	-8.650363	9.064653
-175.252357	-8.855805	9.074650
-173.337155	-14.390830	9.084647
-171.710914	-8.583901	9.094643
-169.548563	-7.596222	9.104640
-167.795552	-11.347986	9.114637
-166.012862	-16.887124	9.124634
-164.144049	-7.409929	9.134631
-162.283126	-11.827859	9.144627
-160.320719	-7.236671	9.154624
-158.339215	-14.277535	9.164621
-156.319836	-9.621224	9.174618
-154.819765	-14.521573	9.184615
-152.791429	-3.628233	9.194611
-150.711005	-2.565885	9.204608
-149.023851	-2.326581	9.214605
-147.374404	-7.803398	9.224602
-145.274596	-8.856781	9.234599
-143.429022	-1.947975	9.244595
-141.638938	1.532299	9.254592
-139.600300	-6.577151	9.264589
-137.957496	-1.811790	9.274586
-135.748933	-4.658843	9.284583
-133.913312	0.268390	9.294579
-132.243612	-1.084256	9.304576
-130.037606	-4.846691	9.314573
-128.317471	3.774785	9.324570
-126.499013	1.567877	9.334567
-124.870197	-3.056157	9.344563
-122.640978	5.056206	9.354560
-120.857359	0.259054	9.364557
-119.209810	4.351038	9.374554
-117.174471	6.693249	9.384551
-115.355723	4.276301	9.394547
-112.997112	-3.361544	9.404544
-111.528040	-3.720583	9.414541
-109.695056	-4.158205	9.424538
-108.173465	-1.405602	9.434535
-105.799865	4.203201	9.444531
-103.876332	-0.109415	9.454528
-102.143024	0.166769	9.464525
-100.414811	5.731698	9.474522
-98.183258	5.994714	9.484519
-96.403113	2.022349	9.494515
-94.615209	4.831951	9.504512
-92.866301	1.390365	9.514509
-90.711158	5.372971	9.524506
-89.060546	1.689699	9.534503
-87.181941	5.373790	9.544499
-85.021248	1.088092	9.554496
-83.533576	11.253019	9.564493
-81.709459	2.629931	9.574490
-79.559424	2.290175	9.584487
-77.638651	2.732262	9.594483
-75.822310	-2.622714	9.604480
-73.935598	5.097491	9.614477
-72.057205	4.491599	9.624474
-70.422637	-4.139135	9.634471
-68.389623	-3.313890	9.644467
-66.515742	-0.666405	9.654464
-64.225919	-1.472134	9.664461
-62.564429	3.533462	9.674458
-60.958728	0.569483	9.684455
-59.232286	-0.242688	9.694451
-56.995718	-1.598867	9.704448
-55.559768	3.510608	9.714445
-53.238889	2.821515	9.724442
-51.276412	6.042254	9.734439
-49.689068	0.250136	9.744435
-47.751796	3.490688	9.754432
-45.935238	-0.345344	9.764429
-43.842572	1.971996	9.774426
-42.082949	3.044558	9.784423
-40.247934	8.379338	9.794419
-38.236655	-4.058337	9.804416
-36.493021	0.375224	9.814413
-34.529657	-1.077883	9.824410
-32.662411	3.705441	9.834407
-30.863924	0.412306	9.844403
-28.983186	-1.594463	9.854400
-27.106008	-4.338037	9.864397
-25.320516	2.299398	9.874394
-23.255725	-2.023056	9.884391
-21.332920	-3.433368	9.894387
-19.463023	-6.090510	9.904384
-17.771688	-2.264388	9.914381
-15.728375	-4.721818	9.924378
-14.022360	0.382502	9.934375
-12.324903	6.145037	9.944371
-10.314851	1.138159	9.954368
-7.922774	1.140390	9.964365
-6.193612	-1.521139	9.974362
-4.853959	0.976339	9.984359
-3.231529	19.382533	9.994355
-2.090311	51.043539	10.004352
-0.825784	105.717376	10.014349
0.000000	160.133632	10.019354
1.211735	190.874038	10.024359
1.335079	229.929970	10.029363
1.971158	261.345817	10.034368
2.357836	284.795225	10.039373
2.450340	302.780068	10.044378
3.077702	316.592109	10.049383
3.388991	337.161455	10.054387
3.542518	341.584081	10.059392
3.295401	340.363526	10.064397
3.358333	362.473801	10.069402
3.653236	375.820097	10.074407
3.261210	388.288774	10.079411
3.825851	373.862415	10.084416
3.700051	382.371407	10.089421
3.812367	402.390673	10.094426
4.416156	406.317297	10.099431
4.273112	416.295654	10.104435
4.400465	417.231032	10.109440
4.470745	424.511843	10.114445
4.532102	415.724591	10.119450
4.100044	403.783222	10.124455
3.955112	420.320560	10.129459
4.073259	425.341801	10.134464
4.356798	432.486099	10.139469
4.400003	441.340338	10.144474
4.737980	436.271650	10.149479
4.720488	440.936052	10.154483
4.773069	439.282905	10.159488
4.595162	445.376413	10.164493
4.766965	450.464800	10.169498
4.624898	450.332951	10.174503
4.457870	452.270938	10.179507
4.572030	447.308907	10.184512
4.737928	455.180046	10.189517
4.608051	462.465990	10.194522
5.094075	463.613832	10.199527
4.972599	482.826808	10.204531
5.257416	483.106279	10.209536
5.379164	487.604983	10.214541
5.266755	488.149664	10.219546
5.440366	473.239934	10.224551
4.970306	469.561702	10.229555
5.491894	472.299788	10.234560
5.565337	490.814619	10.239565
5.357504	486.774430	10.244570
5.591627	482.501323	10.249575
5.569123	482.430831	10.254579
5.473813	479.257390	10.259584
5.515043	488.638689	10.264589
5.846334	498.636069	10.269594
5.761394	488.378693	10.274599
5.314589	490.145259	10.279603
5.418851	503.878479	10.284608
5.718680	502.371976	10.289613
5.709522	507.968652	10.294618
5.775611	505.573731	10.299623
5.776067	511.395962	10.304627
5.886221	518.668884	10.309632
5.582723	519.037456	10.314637
5.722781	522.915068	10.319642
6.089656	518.447309	10.324647
5.993834	532.075268	10.329651
6.327711	545.552704	10.334656
6.075821	540.459782	10.339661
6.325038	547.836699	10.344666
6.382101	545.558333	10.349671
6.185029	572.057395	10.354675
6.270170	553.122991	10.359680
6.506109	564.592773	10.364685
6.169063	562.780973	10.369690
6.604336	552.071564	10.374695
6.431934	567.079030	10.379699
6.325780	564.309435	10.384704
6.535411	566.327717	10.389709
6.165326	566.495592	10.394714
6.578369	563.580111	10.399719
6.600912	579.084792	10.404723
6.922906	585.913940	10.409728
6.989162	590.664385	10.414733
7.000798	611.600467	10.419738
7.164456	605.611742	10.424743
6.764505	617.742821	10.429747
6.917890	616.223392	10.434752
6.915375	609.289731	10.439757
6.956769	617.190278	10.444762
7.242363	606.436891	10.449767
6.959726	617.109453	10.454771
7.071360	614.743522	10.459776
7.019076	611.714582	10.464781
6.895198	622.237244	10.469786
7.281388	613.164668	10.474791
7.049722	626.738686	10.479795
7.397223	636.837659	10.484800
7.513111	646.519401	10.489805
7.498589	640.518076	10.494810
7.527266	643.032024	10.499815
7.580422	646.672785	10.504819
7.461272	646.332267	10.509824
7.652491	649.130963	10.514829
7.514262	655.506823	10.519834
7.765906	643.184966	10.524839
7.768789	656.426702	10.529843
7.461866	654.581700	10.534848
7.670873	668.643735	10.539853
8.199008	681.204034	10.544858
8.104054	673.789903	10.549863
8.343050	681.865558	10.554867
8.389227	680.055704	10.559872
8.238713	689.018264	10.564877
8.096130	687.197511	10.569882
8.237657	678.990271	10.574887
8.124577	691.643384	10.579891
8.133393	693.428773	10.584896
8.451115	696.874381	10.589901
8.347323	694.221084	10.594906
8.343447	690.580410	10.599911
8.038123	701.105259	10.604915
8.086498	693.497941	10.609920
8.396888	699.422209	10.614925
8.038548	721.237505	10.619930
8.698866	722.141520	10.624935
8.739588	734.760678	10.629939
8.763027	737.814819	10.634944
8.714644	732.572673	10.639949
8.861441	726.244374	10.644954
8.912424	725.782098	10.649959
8.438628	743.771070	10.654963
8.949870	732.620463	10.659968
9.267246	740.290972	10.664973
8.838436	750.524878	10.669978
9.377045	758.317815	10.674983
9.277183	771.899332	10.679987
9.413570	762.852311	10.684992
9.156534	750.755002	10.689997
9.477652	768.782812	10.695002
9.543490	777.867046	10.700007
9.289056	775.386000	10.705011
9.651448	770.329073	10.710016
9.420797	776.194578	10.715021
9.376416	779.683763	10.720026
9.397900	775.837165	10.725031
9.386456	786.129114	10.730035
9.659085	780.234907	10.735040
9.565972	777.425343	10.740045
9.312822	791.491817	10.745050
9.766131	780.593276	10.750055
9.404004	785.949873	10.755059
9.594279	786.482561	10.760064
9.980604	805.572394	10.765069
9.804706	816.008871	10.770074
10.078417	817.105446	10.775079
9.793208	823.034866	10.780083
10.063541	818.155039	10.785088
10.455535	824.958943	10.790093
10.354627	825.329905	10.795098
10.194792	815.126823	10.800103
10.041261	828.657026	10.805107
10.315217	829.382960	10.810112
10.665066	823.610467	10.815117
10.236804	830.540464	10.820122
10.336275	825.650037	10.825127
10.344903	830.187390	10.830131
10.228366	830.814747	10.835136
10.435713	835.071237	10.840141
10.222034	839.877450	10.845146
10.924217	843.939899	10.850151
10.696096	859.530591	10.855155
10.999255	861.627043	10.860160
11.127473	866.192645	10.865165
10.526742	866.914575	10.870170
10.880725	858.577151	10.875175
10.807367	864.053309	10.880179
10.836190	873.742780	10.885184
11.063261	865.376705	10.890189
10.707409	871.080856	10.895194
10.943485	866.329486	10.900199
10.872629	880.343317	10.905203
10.794487	877.039311	10.910208
11.125905	877.002260	10.915213
10.937433	887.995910	10.920218
11.321202	901.103002	10.925223
11.267857	899.678019	10.930227
11.013005	908.922297	10.935232
11.613148	903.630276	10.940237
11.440766	908.735870	10.945242
11.535848	903.100177	10.950247
11.472536	909.380617	10.955251
11.334507	903.121323	10.960256
11.761678	909.643675	10.965261
11.516711	908.840643	10.970266
11.468151	908.796382	10.975271
11.923599	924.256044	10.980275
11.777104	930.822587	10.985280
11.901577	931.201764	10.990285
11.755924	942.655430	10.995290
12.405240	941.766541	11.000295
12.099812	948.735354	11.005299
12.132926	945.760538	11.010304
12.245044	938.970873	11.015309
12.231392	950.143280	11.020314
12.438597	943.522962	11.025319
12.119987	947.041731	11.030323
12.513623	946.436484	11.035328
12.581492	947.513857	11.040333
12.032689	955.844627	11.045338
12.323297	939.977420	11.050343
12.309560	947.579416	11.055347
12.358688	956.093960	11.060352
12.259595	954.945943	11.065357
12.277038	959.688523	11.070362
12.475778	944.936739	11.075367
12.096300	963.010292	11.080371
12.104795	977.610837	11.085376
12.605623	981.027310	11.090381
12.271791	995.280324	11.095386
12.955594	992.689029	11.100391
12.678567	991.143584	11.105395
12.628833	992.876843	11.110400
12.827384	1001.837543	11.115405
13.159482	1025.434058	11.120410
13.298131	1017.898912	11.125415
13.011902	1024.129792	11.130419
13.292763	1021.801465	11.135424
13.343606	1020.320428	11.140429
13.130345	1026.951282	11.145434
13.578672	1026.086560	11.150439
13.628888	1025.555006	11.155443
13.629080	1035.477824	11.160448
13.792052	1033.005860	11.165453
13.523267	1023.901865	11.170458
13.376693	1010.859415	11.175463
13.357879	1026.153536	11.180467
13.389750	1032.459851	11.185472
13.794468	1031.097426	11.190477
13.648757	1032.773453	11.195482
13.445980	1032.148200	11.200487
13.797026	1033.204071	11.205491
13.457073	1038.232350	11.210496
13.487596	1026.855395	11.215501
13.303776	1035.727280	11.220506
13.660878	1049.797607	11.225511
13.961766	1057.809981	11.230515
13.865256	1066.308392	11.235520
13.951149	1069.666475	11.240525
13.621970	1065.766910	11.245530
14.060442	1063.809280	11.250535
13.899345	1064.140959	11.255539
13.858903	1072.753441	11.260544
14.409955	1080.219695	11.265549
14.091413	1103.352365	11.270554
14.511617	1103.186030	11.275559
14.314848	1113.181316	11.280563
14.481560	1105.043942	11.285568
14.816984	1103.883387	11.290573
14.333355	1115.780626	11.295578
14.702182	1102.226933	11.300583
14.663575	1108.058787	11.305587
14.567266	1105.156623	11.310592
14.915051	1100.060909	11.315597
14.627539	1109.465075	11.320602
14.530097	1105.812410	11.325607
14.501287	1114.060337	11.330611
14.601328	1125.571162	11.335616
14.995453	1125.470492	11.340621
14.821614	1140.172826	11.345626
14.864935	1138.994195	11.350631
14.893797	1151.093598	11.355635
14.669403	1148.699166	11.360640
14.823902	1150.436143	11.365645
14.583073	1151.983841	11.370650
14.899869	1156.856951	11.375655
15.524218	1174.094105	11.380659
15.277920	1178.995523	11.385664
15.555545	1180.343834	11.390669
15.064977	1183.024273	11.395674
15.581298	1183.941824	11.400679
15.410731	1180.125749	11.405683
15.547574	1181.493358	11.410688
15.744185	1174.906167	11.415693
15.736782	1184.007067	11.420698
15.789806	1180.456552	11.425703
15.743645	1187.871442	11.430707
15.752728	1183.089935	11.435712
16.084118	1185.579354	11.440717
15.928330	1190.191931	11.445722
15.933525	1183.903365	11.450727
15.823826	1191.424592	11.455731
16.145210	1188.116724	11.460736
16.248976	1189.054339	11.465741
16.123724	1185.617416	11.470746
15.964334	1185.824237	11.475751
16.203081	1193.067525	11.480755
16.368199	1205.842307	11.485760
16.435940	1191.089089	11.490765
16.107887	1202.734487	11.495770
16.394535	1210.140468	11.500775
16.478010	1218.397357	11.505779
16.483185	1222.003333	11.510784
16.625819	1234.324375	11.515789
16.465013	1228.044918	11.520794
16.783357	1221.949262	11.525799
16.635280	1225.972372	11.530803
16.594897	1223.398758	11.535808
16.634331	1218.248095	11.540813
16.815095	1224.578059	11.545818
17.020833	1223.890799	11.550823
17.101755	1218.755597	11.555827
16.892701	1219.003458	11.560832
17.104768	1221.056140	11.565837
16.867132	1221.458380	11.570842
17.294198	1224.470329	11.575847
17.071704	1225.354316	11.580851
16.898744	1236.255860	11.585856
17.119370	1231.505259	11.590861
16.831162	1230.860503	11.595866
16.836406	1223.264519	11.600871
17.042553	1231.821996	11.605875
16.925538	1227.000657	11.610880
17.372365	1254.318488	11.615885
17.172896	1269.632214	11.620890
17.299618	1267.844136	11.625895
17.173086	1273.743700	11.630899
17.104421	1273.335185	11.635904
17.351067	1268.613540	11.640909
17.337089	1274.115078	11.645914
17.556508	1278.592142	11.650919
17.653428	1299.766368	11.655923
17.740082	1293.344906	11.660928
17.877536	1290.091583	11.665933
17.607890	1300.772034	11.670938
18.214651	1287.965609	11.675943
18.194224	1292.141858	11.680947
17.757440	1299.619103	11.685952
18.018656	1291.316732	11.690957
17.554241	1292.576800	11.695962
17.880443	1284.440701	11.700967
18.059068	1295.248367	11.705971
17.985792	1300.593778	11.710976
18.323525	1304.577280	11.715981
17.981625	1316.237593	11.720986
18.621216	1325.199123	11.725991
18.581310	1321.903111	11.730995
18.504495	1332.609606	11.736000
18.684812	1317.428263	11.741005
18.372105	1328.006782	11.746010
18.421112	1328.077857	11.751015
18.459302	1329.743513	11.756019
18.654917	1320.973730	11.761024
18.697986	1331.274719	11.766029
18.249742	1333.920047	11.771034
18.510063	1330.673930	11.776039
18.544791	1337.585522	11.781043
18.522499	1338.423393	11.786048
18.786281	1338.564302	11.791053
18.923769	1358.686536	11.796058
18.678825	1360.293263	11.801063
18.926084	1369.441982	11.806067
19.031455	1366.717352	11.811072
19.131657	1366.893813	11.816077
18.693746	1368.676409	11.821082
19.093339	1362.774335	11.826087
18.803488	1373.242000	11.831091
19.320819	1387.447964	11.836096
19.372597	1387.020237	11.841101
19.399378	1396.109510	11.846106
19.326206	1400.063158	11.851111
19.304615	1401.071245	11.856115
19.779923	1401.276989	11.861120
19.674253	1396.523175	11.866125
19.491450	1407.539968	11.871130
19.875057	1393.807014	11.876135
19.864304	1399.352243	11.881139
19.439533	1398.483232	11.886144
19.687513	1395.445669	11.891149
19.670952	1404.859643	11.896154
19.763273	1389.853911	11.901159
19.838627	1403.021685	11.906163
19.750688	1404.690905	11.911168
20.082160	1392.277620	11.916173
19.743136	1406.970293	11.921178
20.204661	1405.870037	11.926183
20.286676	1402.780874	11.931187
20.067310	1411.247035	11.936192
20.440709	1417.914613	11.941197
20.361943	1418.014740	11.946202
20.382881	1422.395760	11.951207
20.247374	1414.764559	11.956211
20.460989	1425.576993	11.961216
20.484078	1425.465316	11.966221
20.285210	1432.463887	11.971226
20.306880	1419.707291	11.976231
20.586556	1427.828131	11.981235
20.347978	1430.880046	11.986240
20.532381	1424.307307	11.991245
20.250415	1435.152261	11.996250
20.533105	1431.308778	12.001255
20.617365	1449.476143	12.006259
20.708705	1460.615638	12.011264
21.101201	1454.380315	12.016269
20.965343	1475.636869	12.021274
21.161668	1468.262619	12.026279
21.088250	1460.258759	12.031283
20.966084	1454.606246	12.036288
21.010678	1440.404508	12.041293
20.723877	1447.477829	12.046298
21.097258	1452.943678	12.051303
21.030677	1455.539197	12.056307
20.741858	1458.272671	12.061312
20.788511	1454.514140	12.066317
21.211361	1466.399568	12.071322
21.213770	1459.401633	12.076327
21.146545	1449.412014	12.081331
20.523569	1443.081582	12.086336
20.808879	1451.296950	12.091341
21.261376	1457.715367	12.096346
21.162887	1453.176453	12.101351
21.347045	1453.140811	12.106355
21.299534	1446.570352	12.111360
21.344711	1436.417722	12.116365
21.136733	1433.791945	12.121370
21.188928	1436.431601	12.126375
21.111886	1430.219129	12.131379
21.067703	1439.566562	12.136384
21.391466	1447.468262	12.141389
21.222242	1447.770491	12.146394
21.493237	1430.825568	12.151399
21.026455	1415.927114	12.156403
20.943764	1417.041150	12.161408
21.191513	1415.590965	12.166413
20.819798	1403.370249	12.171418
21.018184	1408.899475	12.176423
21.326436	1414.412759	12.181427
21.126028	1420.042652	12.186432
21.020016	1414.572887	12.191437
20.875907	1419.974586	12.196442
20.947467	1404.369700	12.201447
21.121215	1404.077863	12.206451
21.216232	1414.578803	12.211456
21.481074	1413.121948	12.216461
20.998373	1414.944811	12.221466
20.838728	1419.228462	12.226471
21.103188	1410.950739	12.231475
21.047837	1418.725212	12.236480
21.395284	1401.839099	12.241485
20.997147	1396.362309	12.246490
20.733327	1384.642477	12.251495
20.968020	1393.110334	12.256499
20.671459	1407.573866	12.261504
20.959644	1415.131897	12.266509
21.115987	1419.018981	12.271514
20.906370	1407.780962	12.276519
21.196798	1420.571432	12.281523
20.924940	1422.263678	12.286528
21.047995	1407.543212	12.291533
20.788388	1406.703057	12.296538
20.797788	1416.235912	12.301543
20.868977	1412.289747	12.306547
20.824811	1425.309431	12.311552
20.914473	1421.730934	12.316557
20.737055	1428.283707	12.321562
20.942470	1424.397352	12.326567
21.169947	1425.304213	12.331571
20.777444	1432.251656	12.336576
20.794337	1420.568246	12.341581
20.831215	1430.388490	12.346586
20.556039	1422.313529	12.351591
20.729035	1428.092050	12.356595
20.898810	1421.490891	12.361600
20.822852	1428.432008	12.366605
21.041371	1424.417395	12.371610
20.695959	1420.428850	12.376615
21.175415	1424.221822	12.381619
20.747380	1431.989502	12.386624
20.946923	1430.834823	12.391629
21.033868	1430.139688	12.396634
21.079575	1427.814894	12.401639
21.489772	1429.283236	12.406643
21.087503	1432.532373	12.411648
21.063922	1434.089610	12.416653
21.080348	1430.511751	12.421658
21.320910	1435.018612	12.426663
21.296179	1437.084646	12.431667
20.941466	1436.090119	12.436672
21.151968	1438.058708	12.441677
20.965811	1443.057076	12.446682
21.004844	1443.447527	12.451687
20.955963	1441.418540	12.456691
20.774451	1434.446795	12.461696
21.227649	1437.337917	12.466701
21.192079	1428.703509	12.471706
20.855217	1417.923419	12.476711
20.925048	1411.103218	12.481715
20.861885	1409.753874	12.486720
20.802871	1416.914653	12.491725
20.956528	1429.802645	12.496730
21.196950	1429.590069	12.501735
21.035571	1418.006062	12.506739
20.706137	1420.630091	12.511744
21.119081	1429.030113	12.516749
20.892776	1430.746637	12.521754
20.906505	1439.886121	12.526759
21.278976	1436.866545	12.531763
20.645087	1423.645165	12.536768
20.864084	1423.838954	12.541773
20.771637	1438.501796	12.546778
20.724837	1443.183022	12.551783
21.077146	1448.519754	12.556787
21.176065	1445.710187	12.561792
21.196655	1443.220647	12.566797
20.749399	1448.055636	12.571802
21.191508	1438.157485	12.576807
21.254731	1442.583023	12.581811
20.946001	1426.166630	12.586816
20.818167	1409.374444	12.591821
20.888475	1416.626572	12.596826
20.673637	1429.326518	12.601831
21.088126	1440.318257	12.606835
21.090767	1446.529268	12.611840
21.187718	1431.907566	12.616845
21.056943	1419.571133	12.621850
21.112709	1402.006075	12.626855
21.014095	1413.684441	12.631859
20.636993	1418.257474	12.636864
20.807787	1411.344681	12.641869
20.806650	1413.417988	12.646874
21.023224	1432.075997	12.651879
20.936218	1438.496073	12.656883
20.800397	1457.231606	12.661888
20.717917	1444.464788	12.666893
20.993528	1455.045774	12.671898
21.197921	1450.242493	12.676903
21.106445	1447.406515	12.681907
21.072003	1461.720266	12.686912
21.230829	1450.749123	12.691917
20.948130	1424.482764	12.696922
20.887216	1424.657322	12.701927
20.776149	1409.586227	12.706931
20.715161	1424.669065	12.711936
20.955322	1434.713170	12.716941
20.838765	1447.686854	12.721946
21.024141	1456.900696	12.726951
21.289511	1462.041544	12.731955
20.791656	1447.371962	12.736960
21.203913	1456.813783	12.741965
21.212797	1448.635940	12.746970
20.696450	1431.162090	12.751975
21.139654	1427.002035	12.756979
21.042119	1423.483358	12.761984
21.053199	1420.608162	12.766989
20.753580	1426.142695	12.771994
20.764917	1436.440145	12.776999
20.958968	1427.579077	12.782003
21.039442	1435.455699	12.787008
21.204793	1428.160532	12.792013
21.028966	1431.069964	12.797018
20.964346	1425.763919	12.802023
21.087417	1427.047008	12.807027
20.839749	1431.541838	12.812032
20.892416	1424.835553	12.817037
20.965711	1436.192391	12.822042
20.745286	1427.768043	12.827047
20.942057	1420.950460	12.832051
20.799306	1427.992911	12.837056
21.110644	1442.390280	12.842061
20.778204	1439.706286	12.847066
20.568700	1451.723306	12.852071
21.182970	1457.149162	12.857075
21.221440	1459.624627	12.862080
21.042403	1458.766888	12.867085
21.356176	1441.119631	12.872090
21.090982	1429.015959	12.877095
20.972635	1428.672138	12.882099
21.032430	1433.360017	12.887104
21.028780	1425.677029	12.892109
21.092692	1432.757492	12.897114
20.768138	1426.755611	12.902119
20.966454	1426.226446	12.907123
20.862078	1433.073528	12.912128
21.020466	1431.395509	12.917133
20.979350	1429.931461	12.922138
21.077057	1431.423619	12.927143
21.173293	1430.215235	12.932147
20.899155	1442.759843	12.937152
21.083349	1429.105973	12.942157
21.005397	1436.602549	12.947162
20.836602	1439.953236	12.952167
21.216838	1428.867943	12.957171
21.311710	1437.122350	12.962176
21.211517	1433.931342	12.967181
21.258088	1435.229787	12.972186
21.173758	1441.293014	12.977191
21.104789	1440.110188	12.982195
21.254974	1437.300332	12.987200
20.785116	1419.665315	12.992205
20.982452	1421.854429	12.997210
20.856953	1426.184680	13.002215
21.159040	1418.843266	13.007219
20.912505	1429.020185	13.012224
21.003130	1419.050359	13.017229
20.802261	1410.585840	13.022234
20.848811	1410.681752	13.027239
20.770686	1420.905931	13.032243
20.839356	1431.873173	13.037248
21.231634	1438.295665	13.042253
20.932808	1438.930829	13.047258
20.964357	1446.960353	13.052263
21.100764	1444.065164	13.057267
21.267422	1439.722108	13.062272
21.219014	1416.017454	13.067277
21.110144	1414.876478	13.072282
20.588455	1414.128588	13.077287
20.934063	1408.657768	13.082291
20.744399	1410.340058	13.087296
20.976266	1407.059824	13.092301
21.102466	1403.603250	13.097306
21.135792	1415.106019	13.102311
21.171672	1405.476911	13.107315
20.905947	1413.906308	13.112320
21.169207	1416.077810	13.117325
21.364526	1411.460509	13.122330
20.792287	1407.161970	13.127335
21.106293	1399.023810	13.132339
20.726255	1416.675351	13.137344
20.927076	1409.884726	13.142349
21.178782	1404.905165	13.147354
21.159374	1406.303235	13.152359
21.218295	1406.151149	13.157363
21.065561	1418.455581	13.162368
21.044365	1409.001958	13.167373
21.207587	1402.466513	13.172378
21.089025	1417.243896	13.177383
21.284825	1409.431327	13.182387
20.998288	1414.871509	13.187392
21.048654	1410.419265	13.192397
21.483665	1417.441325	13.197402
20.948774	1397.241313	13.202407
21.004661	1377.026752	13.207411
20.785771	1383.537229	13.212416
20.882713	1373.858976	13.217421
20.893018	1383.255247	13.222426
20.577234	1399.720011	13.227431
21.011257	1386.045262	13.232435
21.120838	1405.302246	13.237440
21.375721	1397.974679	13.242445
20.844753	1382.927209	13.247450
20.762294	1382.456230	13.252455
20.930308	1384.687864	13.257459
20.926711	1402.817140	13.262464
21.086690	1401.195645	13.267469
20.858422	1388.626395	13.272474
20.829434	1404.540756	13.277479
21.343772	1399.866271	13.282483
20.997554	1395.865244	13.287488
20.827979	1395.466511	13.292493
20.738310	1387.426645	13.297498
20.628098	1392.019399	13.302503
21.363837	1403.273717	13.307507
21.156367	1409.740592	13.312512
20.983999	1396.312367	13.317517
20.836052	1387.802359	13.322522
20.863300	1388.786886	13.327527
21.251983	1392.027363	13.332531
20.835700	1390.619210	13.337536
20.743984	1391.846657	13.342541
21.009876	1398.659905	13.347546
20.980566	1413.829940	13.352551
21.059793	1392.772621	13.357555
20.978848	1401.104725	13.362560
21.140860	1379.141589	13.367565
21.036849	1380.503472	13.372570
21.005322	1385.468485	13.377575
20.861807	1381.340509	13.382579
21.120157	1392.184422	13.387584
20.876795	1396.318978	13.392589
21.091117	1383.868397	13.397594
20.653496	1391.366325	13.402599
21.126929	1387.023248	13.407603
20.877744	1396.282701	13.412608
20.688476	1388.735000	13.417613
20.893375	1399.190805	13.422618
20.657350	1423.033128	13.427623
20.755584	1418.797194	13.432627
20.860616	1422.753181	13.437632
21.038485	1431.012484	13.442637
21.193215	1433.644461	13.447642
20.779223	1429.998829	13.452647
21.294158	1421.955567	13.457651
21.052061	1441.434281	13.462656
20.964946	1423.359715	13.467661
21.139294	1420.926877	13.472666
20.760997	1417.445882	13.477671
20.821561	1422.201450	13.482675
20.825252	1425.589286	13.487680
20.869754	1428.788459	13.492685
21.089068	1421.103821	13.497690
20.753170	1429.824353	13.502695
21.084457	1426.325602	13.507699
20.665944	1439.393961	13.512704
21.083448	1427.320983	13.517709
21.024050	1422.734051	13.522714
20.866272	1426.653886	13.527719
21.195015	1428.241672	13.532723
20.877278	1431.637402	13.537728
20.892682	1428.375126	13.542733
21.358183	1426.187616	13.547738
21.006960	1431.003340	13.552743
20.903265	1418.322726	13.557747
20.999569	1429.339969	13.562752
20.842013	1415.661760	13.567757
21.252155	1419.677905	13.572762
20.610042	1427.547539	13.577767
21.280081	1424.917363	13.582771
21.119169	1427.419891	13.587776
21.030029	1407.482329	13.592781
20.833632	1393.474415	13.597786
21.140625	1397.194740	13.602791
20.880579	1395.785326	13.607795
20.646608	1406.652569	13.612800
20.948781	1413.975747	13.617805
21.770319	1414.827291	13.622810
21.447275	1405.302739	13.627815
21.126201	1400.192159	13.632819
21.408734	1405.218277	13.637824
20.991954	1395.931839	13.642829
21.177658	1392.320684	13.647834
20.720757	1396.975041	13.652839
20.848581	1400.919500	13.657843
20.927444	1401.373779	13.662848
20.857432	1396.839803	13.667853
21.175992	1395.363344	13.672858
21.124246	1401.374045	13.677863
21.203978	1394.348038	13.682867
21.313431	1406.400893	13.687872
20.992433	1406.107530	13.692877
21.115285	1401.557775	13.697882
20.952467	1398.318410	13.702887
21.022261	1386.622648	13.707891
20.765393	1391.495857	13.712896
20.713999	1395.740158	13.717901
21.286366	1394.379352	13.722906
21.041715	1402.933126	13.727911
20.746198	1389.923552	13.732915
20.726859	1391.218311	13.737920
20.890624	1398.655026	13.742925
21.054196	1403.917754	13.747930
20.872842	1409.037570	13.752935
21.048998	1398.932680	13.757939
20.917351	1399.014431	13.762944
20.975470	1398.841970	13.767949
21.192090	1398.939146	13.772954
20.966857	1401.496874	13.777959
21.287655	1405.260735	13.782963
20.914671	1398.661774	13.787968
20.825691	1383.413704	13.792973
20.920475	1383.169946	13.797978
20.634976	1409.231218	13.802983
21.004205	1402.492593	13.807987
21.166789	1406.786356	13.812992
20.927709	1408.133510	13.817997
21.258526	1400.414540	13.823002
20.880461	1400.281679	13.828007
20.893478	1398.169491	13.833011
20.582254	1404.027593	13.838016
20.787907	1410.875687	13.843021
20.862941	1413.432842	13.848026
20.882316	1418.948829	13.853031
21.114192	1411.958479	13.858035
21.068871	1419.329983	13.863040
21.282828	1417.296142	13.868045
21.093092	1416.621478	13.873050
21.001480	1413.990551	13.878055
21.216247	1403.333038	13.883059
20.962842	1410.355278	13.888064
21.064598	1405.713473	13.893069
21.229845	1393.643693	13.898074
20.812012	1398.283933	13.903079
20.918532	1390.122882	13.908083
20.834355	1389.789384	13.913088
20.538669	1394.298169	13.918093
20.992424	1400.042153	13.923098
20.849263	1412.638393	13.928103
21.394877	1412.359008	13.933107
20.751937	1395.590637	13.938112
20.974820	1389.894947	13.943117
21.047480	1392.351544	13.948122
20.915968	1395.927319	13.953127
20.740839	1390.381845	13.958131
21.148329	1404.579323	13.963136
21.215117	1409.767594	13.968141
20.792723	1394.193396	13.973146
20.811141	1393.761527	13.978151
20.901127	1394.624075	13.983155
21.029928	1415.582844	13.988160
20.954021	1421.212595	13.993165
21.333820	1408.323981	13.998170
20.805740	1406.161670	14.003175
20.903049	1389.764935	14.008179
20.875519	1401.004562	14.013184
20.927915	1402.106516	14.018189
21.084249	1394.569189	14.023207
21.101337	1389.935389	14.028224
21.022970	1387.276855	14.033242
21.100645	1390.456258	14.038259
21.033710	1398.760186	14.043277
21.239156	1400.193558	14.048295
21.178559	1393.977054	14.053312
21.050708	1396.196631	14.058330
21.228035	1404.570147	14.063347
20.865995	1400.066024	14.068365
21.358964	1393.822585	14.073383
20.756972	1408.543452	14.078400
21.067211	1395.083597	14.083418
20.743311	1405.349227	14.088435
20.801243	1408.928197	14.093453
20.970996	1416.480213	14.098471
20.829863	1424.066083	14.103488
21.119379	1417.408329	14.108506
21.071843	1418.457320	14.113523
21.244798	1407.630647	14.118541
21.049274	1418.921904	14.123559
21.238361	1431.613213	14.128576
21.193387	1412.792334	14.133594
21.171261	1424.532581	14.138611
20.952749	1446.057999	14.143629
21.399233	1453.675228	14.148647
21.020889	1468.955896	14.153664
21.384930	1458.831763	14.158682
21.443172	1454.563411	14.163699
21.305822	1461.336205	14.168717
21.420152	1461.859932	14.173735
21.173581	1465.639281	14.178752
21.441675	1457.006783	14.183770
21.599380	1464.366470	14.188787
21.376514	1467.893493	14.193805
21.498523	1465.389398	14.198823
21.529233	1463.482689	14.203840
21.494849	1466.739757	14.208858
21.646709	1469.429918	14.213875
21.555879	1462.286945	14.218893
21.783754	1467.862588	14.223911
21.526983	1474.797583	14.228928
21.703988	1494.727817	14.233946
21.748759	1491.193084	14.238963
21.566024	1500.323314	14.243981
22.082527	1495.318811	14.248999
22.039380	1494.635148	14.254016
21.679724	1476.677655	14.259034
21.900160	1481.225696	14.264051
21.614347	1479.283733	14.269069
22.076835	1489.711878	14.274087
21.926995	1496.961750	14.279104
21.941818	1490.840146	14.284122
22.105249	1485.836898	14.289139
21.606315	1484.600628	14.294157
22.138411	1484.256246	14.299175
21.678349	1491.760877	14.304192
21.760843	1499.937994	14.309210
21.943204	1501.916197	14.314227
21.871464	1500.283807	14.319245
22.228296	1498.627113	14.324263
21.942968	1499.636953	14.329280
22.005437	1498.802734	14.334298
21.997536	1501.287137	14.339315
21.818108	1502.944714	14.344333
21.932611	1490.908951	14.349351
21.850430	1496.488434	14.354368
21.785010	1500.037547	14.359386
22.153633	1496.502288	14.364403
21.908584	1502.893502	14.369421
22.402875	1511.868571	14.374439
22.263284	1519.576160	14.379456
22.374321	1522.629930	14.384474
22.177739	1512.155494	14.389491
22.060456	1516.808533	14.394509
22.402557	1521.484267	14.399527
22.530006	1536.567145	14.404544
22.472891	1541.058793	14.409562
22.667466	1534.372081	14.414579
22.245320	1517.629486	14.419597
22.343540	1506.898818	14.424615
22.296579	1527.981703	14.429632
22.527080	1530.808776	14.434650
22.660817	1533.904548	14.439667
22.391422	1535.368043	14.444685
22.651286	1525.680492	14.449703
22.493828	1533.403521	14.454720
22.800013	1532.240984	14.459738
22.592374	1513.922561	14.464755
22.525898	1509.232834	14.469773
22.541031	1524.778007	14.474791
22.533094	1538.385692	14.479808
22.245639	1534.008849	14.484826
22.386730	1540.718395	14.489843
22.538859	1540.543154	14.494861
22.777830	1537.916570	14.499879
22.439977	1541.030923	14.504896
22.734720	1542.446922	14.509914
22.851443	1534.427639	14.514931
22.570811	1544.308139	14.519949
22.584096	1529.449070	14.524967
22.493671	1533.990074	14.529984
22.520507	1539.183299	14.535002
22.907744	1555.410870	14.540019
22.819272	1568.061619	14.545037
23.028205	1566.674693	14.550055
22.974384	1572.325977	14.555072
22.955252	1567.230690	14.560090
23.197761	1574.001945	14.565107
23.152761	1556.449579	14.570125
22.755981	1541.854105	14.575143
22.798996	1556.967774	14.580160
23.018851	1555.020662	14.585178
23.365324	1561.686451	14.590195
22.771598	1561.410716	14.595213
23.235695	1566.946363	14.600231
23.259558	1561.886695	14.605248
23.197218	1570.606855	14.610266
23.128067	1545.373826	14.615283
23.296708	1555.844163	14.620301
22.981513	1544.304765	14.625319
23.047173	1549.704169	14.630336
23.238609	1569.909067	14.635354
23.342419	1554.399221	14.640371
23.356393	1569.242244	14.645389
23.362790	1573.429606	14.650407
23.693247	1569.927160	14.655424
23.458270	1561.053136	14.660442
23.341737	1544.891789	14.665459
23.256373	1542.993356	14.670477
23.327810	1543.328079	14.675495
23.363630	1553.356324	14.680512
23.193784	1568.779243	14.685530
23.548104	1566.016276	14.690547
23.396691	1565.807644	14.695565
23.442330	1563.418750	14.700583
23.757027	1569.038002	14.705600
23.334044	1576.924529	14.710618
23.153373	1571.855790	14.715635
23.068345	1569.449193	14.720653
23.358811	1566.277968	14.725671
23.735780	1568.552345	14.730688
23.391020	1571.061382	14.735706
23.874899	1561.386059	14.740723
23.480707	1567.462087	14.745741
23.743870	1567.537348	14.750759
23.613475	1563.769402	14.755776
23.459444	1565.068204	14.760794
23.555398	1560.233002	14.765811
23.420336	1581.982847	14.770829
24.103867	1588.324322	14.775847
24.056702	1597.418047	14.780864
24.119691	1592.106725	14.785882
24.141546	1564.264338	14.790899
23.866895	1558.929009	14.795917
23.805162	1564.269294	14.800935
24.002338	1556.102670	14.805952
23.801329	1551.102464	14.810970
23.910706	1556.673443	14.815987
23.732975	1572.975406	14.821005
24.018605	1579.593490	14.826023
24.095378	1587.832133	14.831040
23.964755	1591.788085	14.836058
24.347131	1584.641946	14.841075
24.100172	1584.082808	14.846093
24.352337	1581.145787	14.851111
24.116892	1564.370215	14.856128
23.952660	1568.827043	14.861146
24.409729	1571.489783	14.866163
24.103537	1568.441244	14.871181
24.169218	1570.120302	14.876199
24.145197	1576.122352	14.881216
24.310568	1579.251630	14.886234
24.608546	1574.542298	14.891251
24.480660	1563.281337	14.896269
24.331621	1561.934199	14.901287
24.406128	1553.930290	14.906304
24.386855	1558.886261	14.911322
24.214719	1550.721908	14.916339
24.247060	1563.561819	14.921357
24.211630	1559.794459	14.926375
24.832889	1564.568051	14.931392
24.360480	1568.629631	14.936410
24.749082	1569.270076	14.941427
24.478418	1564.041865	14.946445
24.428404	1562.693878	14.951463
24.818815	1549.523915	14.956480
24.506813	1551.588046	14.961498
24.445123	1554.402733	14.966515
24.469317	1561.139584	14.971533
24.408431	1581.184171	14.976551
24.752356	1590.485303	14.981568
24.687321	1603.287294	14.986586
24.851744	1591.866430	14.991603
24.765429	1590.177363	14.996621
24.589416	1592.805788	15.001639
24.833520	1588.557308	15.006656
24.671662	1586.955798	15.011674
24.713457	1594.079983	15.016691
24.658191	1592.080785	15.021709
24.656830	1593.264003	15.026727
24.923525	1595.370347	15.031744
24.711754	1598.065040	15.036762
24.895399	1594.415322	15.041779
24.951585	1593.263548	15.046797
24.631323	1590.623105	15.051815
24.855752	1586.669571	15.056832
24.490279	1597.191300	15.061850
24.851548	1593.741352	15.066867
24.802121	1593.963999	15.071885
25.207321	1611.270267	15.076903
25.486860	1617.285272	15.081920
25.078626	1613.884894	15.086938
25.122060	1597.619321	15.091955
25.208773	1589.568614	15.096973
24.730503	1592.670764	15.101991
25.032866	1607.143777	15.107008
25.077162	1622.777216	15.112026
25.061724	1619.463636	15.117043
25.402875	1615.754185	15.122061
25.418701	1621.642143	15.127079
25.509031	1616.720512	15.132096
25.253989	1623.484621	15.137114
25.440343	1620.650114	15.142131
25.495412	1621.191164	15.147149
25.226741	1627.697888	15.152167
25.305247	1624.703607	15.157184
25.168396	1630.715809	15.162202
25.398280	1620.957467	15.167219
25.514984	1622.807726	15.172237
25.091441	1620.466120	15.177255
25.288086	1618.026390	15.182272
25.367770	1628.006005	15.187290
25.381465	1621.134161	15.192307
25.740066	1625.421103	15.197325
25.569847	1619.267605	15.202343
25.636754	1611.711636	15.207360
25.699256	1620.667543	15.212378
25.712300	1622.162298	15.217395
25.616632	1612.507794	15.222413
25.181424	1616.771102	15.227431
25.556379	1634.402346	15.232448
25.767569	1646.820533	15.237466
26.012686	1647.189696	15.242483
26.103266	1651.728613	15.247501
25.918261	1644.610009	15.252519
25.958633	1620.686287	15.257536
25.770766	1611.756740	15.262554
25.709314	1620.359593	15.267571
26.296422	1635.075097	15.272589
25.958238	1632.528744	15.277607
26.137506	1617.065002	15.282624
25.786595	1615.355994	15.287642
25.701734	1620.073111	15.292659
26.016564	1640.257641	15.297677
26.049479	1652.228404	15.302695
26.355494	1647.645975	15.307712
26.237010	1647.963796	15.312730
26.310481	1645.219649	15.317747
26.209872	1638.131635	15.322765
26.107109	1635.535937	15.327783
26.455303	1635.917764	15.332800
26.196187	1632.864062	15.337818
26.218948	1622.095792	15.342835
26.405796	1623.433047	15.347853
26.125758	1623.794724	15.352871
26.227947	1635.340701	15.357888
26.557054	1643.733410	15.362906
26.408128	1636.062405	15.367923
26.521017	1625.247510	15.372941
26.224860	1620.515722	15.377959
26.422882	1624.600962	15.382976
26.371440	1641.403554	15.387994
26.471360	1641.628339	15.393011
26.489582	1637.737567	15.398029
26.157492	1648.095125	15.403047
26.349365	1646.739229	15.408064
26.662797	1651.826223	15.413082
26.565864	1651.466536	15.418099
26.711400	1650.217920	15.423117
26.524914	1649.033269	15.428135
26.665673	1646.413676	15.433152
26.669121	1652.608801	15.438170
26.424533	1657.058807	15.443187
26.440489	1650.452442	15.448205
26.366203	1650.214204	15.453223
26.739571	1654.266768	15.458240
26.707130	1657.037482	15.463258
26.654204	1650.261983	15.468275
27.128291	1645.601624	15.473293
26.514657	1654.557628	15.478311
26.621393	1645.686472	15.483328
26.616385	1663.464082	15.488346
26.873771	1684.600121	15.493363
26.989328	1678.352256	15.498381
26.935339	1696.553803	15.503399
27.011249	1676.586963	15.508416
27.179570	1682.631532	15.513434
27.320385	1693.457208	15.518451
27.348224	1676.225006	15.523469
27.077726	1692.873820	15.528487
27.383821	1680.794760	15.533504
27.430560	1676.739760	15.538522
27.263623	1659.462345	15.543539
27.348115	1653.549009	15.548557
27.149395	1652.451255	15.553575
27.499467	1648.760824	15.558592
27.380344	1642.665237	15.563610
27.337691	1654.759744	15.568627
27.308977	1651.883234	15.573645
27.141480	1648.982453	15.578663
27.110739	1646.717415	15.583680
27.290823	1650.927438	15.588698
27.477829	1674.165331	15.593715
27.823818	1666.822813	15.598733
27.696770	1661.666835	15.603751
27.861029	1652.960328	15.608768
27.456947	1653.095598	15.613786
27.473922	1647.405400	15.618803
27.439417	1644.693418	15.623821
27.188857	1650.811856	15.628839
27.436815	1659.177402	15.633856
27.544343	1663.866210	15.638874
27.497961	1682.838917	15.643891
27.775367	1679.793239	15.648909
27.623898	1683.352973	15.653927
27.509893	1690.410813	15.658944
27.797613	1682.806220	15.663962
27.812321	1687.929070	15.668979
27.920581	1679.211029	15.673997
27.837891	1688.015519	15.679015
27.918154	1683.590998	15.684032
27.796538	1680.041854	15.689050
27.857564	1690.007183	15.694067
27.715432	1680.647922	15.699085
27.804151	1681.860040	15.704103
27.761821	1684.855717	15.709120
27.814829	1681.141865	15.714138
27.464368	1687.352546	15.719155
27.939132	1675.522669	15.724173
27.716117	1684.177283	15.729191
27.626344	1704.943193	15.734208
28.143959	1705.668468	15.739226
28.063509	1720.916834	15.744243
28.597680	1711.319127	15.749261
28.260166	1716.358153	15.754279
28.362395	1710.628378	15.759296
28.583671	1711.460691	15.764314
28.189213	1714.229374	15.769331
28.545100	1704.192893	15.774349
28.111338	1693.952002	15.779367
28.186309	1700.005960	15.784384
28.326295	1703.479889	15.789402
28.279457	1713.305913	15.794419
28.638126	1713.811920	15.799437
28.605715	1718.995780	15.804455
28.337546	1703.825898	15.809472
28.451862	1711.758948	15.814490
28.569421	1708.627854	15.819507
28.782250	1714.881639	15.824525
28.654278	1713.583039	15.829543
28.854578	1708.072802	15.834560
28.892653	1706.078366	15.839578
28.800417	1686.301146	15.844595
28.571213	1672.354460	15.849613
28.543607	1677.638218	15.854631
28.514223	1690.533705	15.859648
28.981412	1700.025259	15.864666
28.911762	1706.289482	15.869683
29.194330	1686.818233	15.874701
28.849131	1676.442102	15.879719
28.636978	1669.868174	15.884736
28.750507	1677.763576	15.889754
28.543680	1688.945154	15.894771
28.896654	1701.771020	15.899789
28.894159	1704.672254	15.904807
28.846308	1706.194032	15.909824
28.397954	1695.924792	15.914842
28.574758	1703.876188	15.919859
28.866929	1700.600838	15.924877
28.779507	1698.126171	15.929895
28.563660	1711.907182	15.934912
29.144178	1724.327099	15.939930
29.091468	1735.669760	15.944947
29.134578	1732.195798	15.949965
29.168009	1728.628995	15.954983
29.118425	1722.936011	15.960000
29.433107	1724.910447	15.965018
29.056129	1731.937097	15.970035
29.173803	1728.633725	15.975053
29.370556	1724.808843	15.980071
28.957327	1738.798331	15.985088
29.348974	1732.385283	15.990106
29.447041	1740.340603	15.995123
29.429907	1737.135811	16.000141
29.429869	1740.005198	16.005159
29.484901	1738.144914	16.010176
29.420130	1738.245734	16.015194
29.302715	1739.398705	16.020211
29.623903	1725.367338	16.025229
29.763727	1730.317657	16.030247
29.382508	1737.619493	16.035264
29.562837	1727.935054	16.040282
29.520573	1738.209487	16.045299
29.518669	1756.203017	16.050317
29.660934	1758.685539	16.055335
29.610344	1759.436937	16.060352
29.621584	1757.517563	16.065370
29.717754	1779.416452	16.070387
29.747029	1769.847316	16.075405
29.700321	1764.717816	16.080423
29.563846	1765.232788	16.085440
30.168312	1763.512977	16.090458
29.615695	1767.317614	16.095475
29.872937	1760.394278	16.100493
29.948384	1760.808594	16.105511
29.855186	1772.002789	16.110528
30.466556	1758.594469	16.115546
29.980174	1770.269028	16.120563
30.287792	1758.350905	16.125581
30.441681	1761.672399	16.130599
30.087674	1781.853676	16.135616
30.464253	1766.300104	16.140634
30.426495	1775.895047	16.145651
30.204953	1768.783782	16.150669
30.306034	1768.486112	16.155687
29.941926	1769.536849	16.160704
30.177607	1769.455252	16.165722
30.180631	1770.144615	16.170739
30.307002	1764.734242	16.175757
30.427774	1759.198129	16.180775
30.052922	1767.917907	16.185792
30.647068	1760.929829	16.190810
30.223981	1771.401879	16.195827
30.155692	1780.521897	16.200845
30.797600	1786.027699	16.205863
30.649098	1802.304806	16.210880
30.947570	1787.028738	16.215898
30.642129	1791.428711	16.220915
30.570836	1789.111127	16.225933
30.850414	1788.935222	16.230951
30.635635	1792.483056	16.235968
30.679257	1793.153360	16.240986
30.440165	1784.345139	16.246003
30.646057	1796.193260	16.251021
30.736216	1793.996227	16.256039
30.434388	1800.301451	16.261056
30.696306	1792.445285	16.266074
30.649617	1794.664563	16.271091
30.805599	1796.042939	16.276109
30.988766	1793.130251	16.281127
30.914454	1801.535477	16.286144
31.318304	1796.319953	16.291162
30.969868	1796.989859	16.296179
31.149191	1798.671270	16.301197
31.270451	1786.247200	16.306215
31.243676	1787.810460	16.311232
31.234387	1796.086542	16.316250
31.182749	1800.884940	16.321267
31.267470	1788.478494	16.326285
31.104128	1782.964086	16.331303
30.928787	1789.481167	16.336320
31.006883	1792.032134	16.341338
30.938931	1783.422361	16.346355
30.805461	1795.371797	16.351373
31.206135	1812.185070	16.356391
31.306023	1821.074574	16.361408
31.616516	1818.334282	16.366426
31.675072	1822.205067	16.371443
31.599679	1819.949483	16.376461
31.736179	1812.722890	16.381479
31.794311	1820.925310	16.386496
31.449905	1813.027396	16.391514
31.491709	1812.762776	16.396531
31.850557	1819.160069	16.401549
31.700969	1822.322325	16.406567
31.616590	1815.233996	16.411584
31.612343	1815.871034	16.416602
31.525504	1826.037800	16.421619
31.561210	1821.485055	16.426637
31.613998	1818.106276	16.431655
31.435392	1824.649850	16.436672
31.749319	1821.625849	16.441690
32.283314	1823.384414	16.446707
32.015117	1821.774667	16.451725
32.035459	1815.902171	16.456743
31.973851	1822.276853	16.461760
31.966073	1822.114526	16.466778
32.006297	1818.094347	16.471795
31.806505	1828.449811	16.476813
32.034577	1817.765063	16.481831
32.074937	1824.607217	16.486848
32.131568	1817.866079	16.491866
31.856995	1812.389063	16.496883
31.681082	1821.000850	16.501901
32.383826	1822.894534	16.506919
31.786710	1824.003672	16.511936
32.358364	1837.577407	16.516954
32.252672	1850.482059	16.521971
32.413811	1851.430157	16.526989
32.383812	1841.890091	16.532007
32.126707	1852.990931	16.537024
32.184894	1851.270922	16.542042
32.344406	1847.305648	16.547059
32.570527	1851.875711	16.552077
32.668239	1854.224561	16.557095
32.544224	1856.765297	16.562112
32.595937	1847.636938	16.567130
32.647940	1841.758596	16.572147
32.785329	1851.633988	16.577165
33.104281	1836.082453	16.582183
32.822197	1840.751651	16.587200
32.661503	1836.142129	16.592218
32.874064	1841.581924	16.597235
32.749868	1840.705092	16.602253
33.150600	1827.922580	16.607271
33.132875	1814.544533	16.612288
33.012070	1797.461742	16.617306
32.994273	1790.340782	16.622323
32.994202	1798.178072	16.627341
33.216462	1797.533082	16.632359
32.908039	1791.683138	16.637376
32.717482	1799.112695	16.642394
33.073046	1796.963002	16.647411
33.236805	1795.171891	16.652429
33.186276	1790.909776	16.657447
32.990325	1797.902868	16.662464
32.839286	1799.571681	16.667482
33.220064	1786.275620	16.672499
33.105037	1808.403300	16.677517
33.166970	1812.078477	16.682535
33.309341	1827.935610	16.687552
33.594831	1827.418183	16.692570
33.426449	1820.926086	16.697587
33.183669	1820.158620	16.702605
33.079778	1820.493782	16.707623
33.225590	1827.447328	16.712640
33.371143	1831.105241	16.717658
33.502358	1828.198472	16.722675
33.236855	1828.651435	16.727693
33.236643	1826.863660	16.732711
33.234797	1828.782405	16.737728
33.064696	1832.275930	16.742746
33.597954	1837.618172	16.747763
33.740628	1855.477863	16.752781
34.282204	1848.222047	16.757799
34.102391	1838.140339	16.762816
33.859785	1828.496540	16.767834
34.227199	1820.695112	16.772851
34.002818	1820.335295	16.777869
33.819171	1819.753465	16.782887
34.245167	1811.742913	16.787904
34.160616	1822.131120	16.792922
34.104884	1823.292351	16.797939
33.928873	1822.208266	16.802957
34.023678	1819.124038	16.807975
34.011778	1820.286931	16.812992
34.060145	1827.299278	16.818010
34.249932	1822.971299	16.823027
34.019268	1824.751920	16.828045
34.022579	1818.855396	16.833063
33.955191	1821.688347	16.838080
33.831316	1814.175283	16.843098
34.188001	1816.480466	16.848115
34.181045	1812.611753	16.853133
34.124541	1816.171319	16.858151
33.855640	1825.461792	16.863168
33.970866	1830.793617	16.868186
34.189188	1831.196162	16.873203
34.305005	1847.932204	16.878221
34.485998	1842.169365	16.883239
34.517138	1843.304945	16.888256
34.490491	1854.513760	16.893274
34.616450	1859.571734	16.898291
34.603134	1861.650411	16.903309
34.817289	1852.379732	16.908327
34.793665	1856.548366	16.913344
34.745530	1853.575807	16.918362
35.073166	1845.783069	16.923379
35.015317	1853.840401	16.928397
34.870418	1849.892211	16.933415
34.919317	1838.878924	16.938432
34.623032	1838.001220	16.943450
34.894024	1838.547171	16.948467
34.619375	1847.933749	16.953485
35.066840	1847.986701	16.958503
34.947893	1852.683372	16.963520
34.421965	1861.526406	16.968538
34.978993	1854.231154	16.973555
34.843612	1854.310200	16.978573
34.710933	1850.296349	16.983591
34.823485	1852.301466	16.988608
34.757365	1845.832377	16.993626
34.978805	1855.042311	16.998643
34.980736	1867.225843	17.003661
35.325239	1869.544777	17.008679
35.081234	1875.547424	17.013696
35.031554	1871.226945	17.018714
35.384985	1862.478347	17.023731
35.093278	1869.422246	17.028749
35.150025	1874.805101	17.033767
35.125512	1875.400540	17.038784
35.173680	1871.644150	17.043802
35.344256	1875.518322	17.048819
35.538292	1897.962599	17.053837
35.814494	1905.376764	17.058855
35.571661	1898.533114	17.063872
35.426859	1914.116008	17.068890
35.835156	1907.102442	17.073907
35.688067	1905.240548	17.078925
35.895286	1907.711951	17.083943
35.995261	1896.796661	17.088960
35.952954	1883.763839	17.093978
35.775320	1875.297353	17.098995
35.732819	1871.169223	17.104013
35.870195	1890.908107	17.109031
36.510084	1885.986838	17.114048
35.828528	1887.096860	17.119066
36.355270	1875.271906	17.124083
36.264017	1872.445441	17.129101
36.154380	1879.022874	17.134119
36.417164	1872.330637	17.139136
36.066454	1873.966804	17.144154
36.211664	1869.538161	17.149171
36.092354	1863.713874	17.154189
36.178795	1867.155482	17.159207
36.551619	1863.465302	17.164224
36.144041	1872.549033	17.169242
36.474805	1861.250090	17.174259
36.448201	1869.932482	17.179277
36.186926	1865.201342	17.184295
36.283188	1867.291648	17.189312
35.992913	1875.751021	17.194330
36.241560	1874.489090	17.199347
36.577595	1895.792230	17.204365
36.523430	1899.497744	17.209383
36.845631	1896.254531	17.214400
36.532610	1905.969755	17.219418
36.615654	1903.488318	17.224435
36.499709	1907.324816	17.229453
36.708470	1906.232061	17.234471
36.966380	1893.397546	17.239488
36.530674	1909.428761	17.244506
36.335802	1896.330590	17.249523
36.892060	1901.282988	17.254541
36.820094	1903.670704	17.259559
36.624350	1888.201983	17.264576
36.372447	1903.708346	17.269594
36.342534	1900.186212	17.274611
36.727865	1911.983788	17.279629
36.618018	1926.259360	17.284647
36.780993	1919.514588	17.289664
36.682738	1934.675563	17.294682
36.940963	1923.822324	17.299699
36.979987	1938.842638	17.304717
37.203953	1938.081746	17.309735
38.236947	1931.615099	17.314752
37.890200	1918.628437	17.319770
37.966844	1911.087277	17.324787
38.143480	1909.474222	17.329805
37.922910	1903.330206	17.334823
37.645420	1883.804857	17.339840
37.753017	1881.021401	17.344858
37.815497	1875.260146	17.349875
37.749406	1879.815468	17.354893
37.500639	1867.197067	17.359911
37.698601	1867.709047	17.364928
37.629204	1874.812561	17.369946
37.888248	1865.183122	17.374963
37.930802	1877.313778	17.379981
37.651455	1875.360502	17.384999
37.799997	1868.346692	17.390016
37.446830	1878.618893	17.395034
37.892798	1874.802994	17.400051
38.002055	1886.724021	17.405069
37.725970	1883.519592	17.410087
37.879725	1874.756424	17.415104
37.738874	1876.969493	17.420122
37.573872	1867.807251	17.425139
37.815623	1879.458589	17.430157
37.799187	1876.425125	17.435175
38.319942	1890.901348	17.440192
38.104780	1904.850755	17.445210
38.192741	1903.531072	17.450227
37.896016	1903.310212	17.455245
37.765211	1906.290155	17.460263
38.117301	1903.274209	17.465280
37.981112	1909.492499	17.470298
38.100956	1911.522418	17.475315
38.326633	1904.481344	17.480333
38.378299	1910.186727	17.485351
38.271278	1900.499233	17.490368
38.237225	1915.547696	17.495386
38.363459	1925.115798	17.500403
38.552783	1927.649051	17.505421
38.488057	1936.283288	17.510439
38.885444	1935.975330	17.515456
38.727967	1938.777836	17.520474
38.396629	1941.801565	17.525491
38.881593	1934.253481	17.530509
38.545327	1942.282899	17.535527
38.609787	1933.522924	17.540544
38.577936	1934.165156	17.545562
38.667601	1937.644022	17.550579
38.680525	1938.092699	17.555597
38.348838	1950.253995	17.560615
39.047356	1959.833894	17.565632
39.139780	1971.431250	17.570650
39.183692	1969.206170	17.575667
39.443329	1963.602213	17.580685
39.110471	1973.844498	17.585703
39.331394	1961.710359	17.590720
39.404590	1959.394088	17.595738
39.022514	1954.424191	17.600755
39.394405	1954.619767	17.605773
39.217559	1963.399324	17.610791
39.487836	1961.352878	17.615808
39.426666	1967.060546	17.620826
38.931932	1964.280318	17.625843
39.320228	1967.908994	17.630861
38.900828	1964.142984	17.635879
39.138780	1970.483329	17.640896
39.263068	1973.161464	17.645914
39.427970	1968.421317	17.650931
39.438616	1962.481878	17.655949
39.411022	1977.583648	17.660967
39.830207	1977.459415	17.665984
39.763254	1993.158188	17.671002
39.722568	1999.808056	17.676019
40.018641	1998.036721	17.681037
40.050083	1997.485867	17.686055
39.719727	2003.934949	17.691072
40.053541	2001.558232	17.696090
40.188047	1998.595845	17.701107
40.387630	1985.588068	17.706125
39.911950	1985.912519	17.711143
40.085512	1966.821675	17.716160
40.120869	1977.559769	17.721178
40.102938	1995.239951	17.726195
40.303744	1988.988584	17.731213
40.043575	1996.099771	17.736231
40.023200	1990.422474	17.741248
40.100674	1998.844509	17.746266
40.132053	1998.390412	17.751283
40.546935	1996.180891	17.756301
39.814728	1996.515576	17.761319
40.342121	2000.947186	17.766336
40.141012	1999.750678	17.771354
40.011760	2005.295387	17.776371
40.341198	2004.630151	17.781389
40.327403	2020.962315	17.786407
40.521033	2023.125211	17.791424
40.811793	2025.717028	17.796442
40.930525	2028.204923	17.801459
41.148646	2025.240995	17.806477
41.039199	2032.754482	17.811495
40.954381	2023.861733	17.816512
41.329380	2021.817455	17.821530
41.065573	2019.677624	17.826547
41.152033	1999.725963	17.831565
40.870570	1997.278257	17.836583
40.659653	1999.871419	17.841600
40.802298	2006.715437	17.846618
40.803394	2015.245622	17.851635
41.368954	2019.664072	17.856653
40.861879	2028.191930	17.861671
40.945135	2021.704448	17.866688
41.042886	2021.542594	17.871706
40.658016	2033.098918	17.876723
40.805772	2032.199940	17.881741
40.958685	2033.327914	17.886759
41.069642	2054.977091	17.891776
41.253294	2058.729667	17.896794
41.275124	2059.213896	17.901811
41.619075	2057.473462	17.906829
41.208425	2056.427564	17.911847
41.409907	2062.684884	17.916864
41.901221	2046.762693	17.921882
41.666776	2049.332085	17.926899
41.823054	2046.593535	17.931917
41.731872	2046.111788	17.936935
41.941284	2041.584759	17.941952
41.951281	2044.008981	17.946970
41.672835	2049.287256	17.951987
41.970214	2051.693965	17.957005
41.917589	2050.602770	17.962023
41.760610	2050.185790	17.967040
42.057368	2047.383148	17.972058
41.807716	2055.774008	17.977075
41.980197	2056.774585	17.982093
41.940836	2055.265179	17.987111
41.910910	2048.068944	17.992128
42.112950	2059.632371	17.997146
42.112990	2083.292447	18.002163
42.560878	2066.751836	18.007181
42.504011	2079.467206	18.012199
42.481292	2077.342405	18.017216
42.584384	2069.090605	18.022234
42.070492	2067.031551	18.027251
42.175219	2066.141006	18.032269
42.314572	2076.746963	18.037287
42.445456	2076.815796	18.042304
42.493249	2073.632038	18.047322
42.513226	2087.994038	18.052339
42.621976	2072.400264	18.057357
42.454633	2072.926461	18.062375
42.374765	2073.750976	18.067392
42.597708	2072.093550	18.072410
42.327106	2081.475698	18.077427
42.638232	2093.804394	18.082445
43.006957	2106.193133	18.087463
43.086028	2106.048416	18.092480
43.209886	2111.842259	18.097498
43.132912	2113.203544	18.102515
43.350902	2101.832733	18.107533
43.260193	2101.862967	18.112551
43.228698	2113.034998	18.117568
43.394897	2103.875635	18.122586
42.934013	2102.674925	18.127603
43.300325	2099.041573	18.132621
43.255363	2107.247224	18.137639
43.513915	2094.689304	18.142656
43.522732	2095.210219	18.147674
43.419499	2110.526338	18.152691
43.143503	2101.019826	18.157709
43.220857	2108.395015	18.162727
43.513973	2108.655857	18.167744
43.666974	2102.275202	18.172762
43.334753	2106.617400	18.177779
43.499635	2098.224372	18.182797
43.595874	2110.197998	18.187815
43.367288	2105.115475	18.192832
43.145107	2101.398207	18.197850
43.289027	2119.845594	18.202867
43.771895	2115.501466	18.207885
43.936422	2119.947720	18.212903
43.561968	2140.307370	18.217920
43.778046	2129.374964	18.222938
44.094868	2133.079580	18.227955
43.971444	2137.168248	18.232973
44.109986	2128.095084	18.237991
43.902002	2127.465994	18.243008
44.299355	2132.153569	18.248026
43.764547	2133.484828	18.253043
44.284739	2129.171713	18.258061
44.374559	2131.190719	18.263079
44.116699	2139.711934	18.268096
44.335869	2142.545655	18.273114
44.327514	2162.935836	18.278131
44.608032	2162.607970	18.283149
44.644907	2164.897354	18.288167
44.601374	2170.938944	18.293184
44.857471	2162.103436	18.298202
44.655761	2164.265687	18.303219
44.856208	2165.948493	18.308237
44.600756	2164.669394	18.313255
44.575690	2168.559899	18.318272
44.755818	2156.748308	18.323290
44.667296	2173.144474	18.328307
44.922222	2162.394627	18.333325
44.716490	2157.120449	18.338343
44.768318	2161.354221	18.343360
44.897080	2159.722031	18.348378
44.852523	2155.012868	18.353395
45.339806	2156.287319	18.358413
45.154774	2151.630449	18.363431
44.788581	2160.699104	18.368448
45.032159	2146.232936	18.373466
45.440879	2160.761907	18.378483
45.168759	2169.976026	18.383501
45.092471	2170.294207	18.388519
45.320074	2183.723348	18.393536
45.335888	2181.023691	18.398554
45.148610	2195.759437	18.403571
45.232305	2183.690261	18.408589
45.330084	2179.800815	18.413607
45.382312	2188.349691	18.418624
45.378846	2182.882785	18.423642
45.182065	2194.795449	18.428659
45.479943	2209.988712	18.433677
45.628748	2216.118420	18.438695
45.747766	2219.410186	18.443712
46.084199	2209.397702	18.448730
46.078279	2226.100105	18.453747
46.034724	2214.951829	18.458765
46.630431	2216.777690	18.463783
46.358642	2208.263886	18.468800
46.179012	2184.349153	18.473818
46.206766	2179.549793	18.478835
45.943488	2187.663666	18.483853
45.888912	2180.914139	18.488871
46.220892	2197.330583	18.493888
46.354710	2207.718849	18.498906
46.025311	2213.924818	18.503923
46.479631	2219.640047	18.508941
46.653547	2212.325486	18.513959
46.674797	2221.070460	18.518976
46.916002	2211.433414	18.523994
46.545448	2188.972042	18.529011
46.332529	2188.434979	18.534029
46.574489	2199.794721	18.539047
46.416395	2207.209081	18.544064
46.749744	2209.252188	18.549082
46.417680	2217.034886	18.554099
46.759268	2213.974145	18.559117
46.953148	2202.242916	18.564135
46.554027	2213.224305	18.569152
46.748824	2209.942349	18.574170
46.572387	2205.788288	18.579187
46.520781	2212.989811	18.584205
46.881899	2220.929403	18.589223
47.137849	2235.694401	18.594240
47.531277	2235.273803	18.599258
47.580143	2239.077025	18.604275
47.189725	2222.109883	18.609293
47.367104	2220.618596	18.614311
47.029735	2230.287576	18.619328
47.163145	2240.064758	18.624346
47.313780	2233.585314	18.629363
47.491416	2239.086677	18.634381
47.942259	2237.775953	18.639399
47.501899	2244.816100	18.644416
47.775050	2240.901030	18.649434
47.671470	2238.288049	18.654451
47.498364	2237.695081	18.659469
47.755528	2229.711228	18.664487
47.571725	2239.176384	18.669504
47.560823	2237.596348	18.674522
47.422569	2240.778123	18.679539
47.650237	2228.284794	18.684557
47.703049	2226.110171	18.689575
47.764820	2248.491132	18.694592
48.047527	2254.697825	18.699610
48.358725	2262.018496	18.704627
48.060525	2270.147422	18.709645
48.374204	2262.639073	18.714663
48.214797	2264.659301	18.719680
48.154292	2261.973374	18.724698
48.093731	2266.751323	18.729715
48.278359	2266.580332	18.734733
48.405925	2259.384047	18.739751
48.206410	2263.132496	18.744768
48.417955	2256.619731	18.749786
48.466706	2264.288236	18.754803
48.082278	2259.150279	18.759821
48.563122	2254.209420	18.764839
48.580950	2255.838768	18.769856
48.353061	2260.757454	18.774874
48.762015	2261.418288	18.779891
48.657328	2258.022046	18.784909
48.719962	2269.255483	18.789927
48.778677	2283.967820	18.794944
48.781076	2280.684281	18.799962
48.760371	2282.885330	18.804979
48.779538	2288.636946	18.809997
48.775266	2277.010408	18.815015
48.672596	2282.857750	18.820032
48.674577	2282.667905	18.825050
48.940030	2287.958636	18.830067
49.414860	2310.584521	18.835085
49.734285	2298.066274	18.840103
49.667718	2309.482383	18.845120
49.320889	2285.502904	18.850138
49.586502	2278.253919	18.855155
49.446517	2284.056871	18.860173
49.738366	2282.567774	18.865191
49.381463	2286.151762	18.870208
49.689754	2286.812132	18.875226
49.926078	2295.650278	18.880243
49.676936	2293.405024	18.885261
49.817656	2298.261793	18.890279
50.030223	2300.044938	18.895296
49.920849	2291.447763	18.900314
50.054137	2278.043635	18.905331
49.832855	2292.628371	18.910349
50.128322	2297.960728	18.915367
50.015266	2297.401443	18.920384
50.041715	2295.809938	18.925402
50.167263	2292.904768	18.930419
50.265675	2292.981928	18.935437
50.458098	2283.465882	18.940455
50.455477	2289.018034	18.945472
50.702730	2286.218524	18.950490
50.442372	2266.523959	18.955507
50.202789	2273.165553	18.960525
50.595966	2273.139072	18.965543
50.593690	2279.399089	18.970560
50.503543	2279.800501	18.975578
50.593860	2284.762839	18.980595
50.510574	2291.989905	18.985613
50.755051	2288.477406	18.990631
50.554641	2299.727645	18.995648
50.936794	2299.184564	19.000666
50.874548	2291.752668	19.005683
50.672252	2302.171005	19.010701
50.914155	2290.258212	19.015719
50.719891	2297.115192	19.020736
50.712281	2295.466979	19.025754
50.848453	2289.995856	19.030771
51.127712	2297.747180	19.035789
51.094908	2286.298233	19.040807
50.864207	2291.780570	19.045824
51.328835	2312.654007	19.050842
51.406868	2312.858696	19.055859
51.287687	2328.959452	19.060877
51.343080	2324.104508	19.065895
51.324243	2325.935571	19.070912
51.507749	2318.861696	19.075930
51.490795	2323.989819	19.080947
51.209374	2327.595602	19.085965
51.404089	2325.677572	19.090983
51.296668	2317.810020	19.096000
51.277220	2319.335985	19.101018
51.548219	2337.143554	19.106035
51.503926	2341.873311	19.111053
51.590934	2351.850682	19.116071
51.745113	2363.379508	19.121088
51.755693	2363.690919	19.126106
51.780410	2358.574204	19.131123
51.689446	2365.132358	19.136141
51.930486	2368.061747	19.141159
51.977075	2383.927682	19.146176
52.171339	2397.455941	19.151194
52.314129	2385.650907	19.156211
52.141941	2389.808775	19.161229
52.286627	2387.429908	19.166247
52.573795	2389.352979	19.171264
52.301809	2381.119915	19.176282
52.474825	2385.020579	19.181299
52.591436	2390.740177	19.186317
52.749903	2383.472830	19.191335
52.590563	2384.154292	19.196352
52.320648	2388.774526	19.201370
52.635629	2385.459207	19.206387
52.917930	2400.907649	19.211405
53.038478	2406.812260	19.216423
53.209587	2396.381591	19.221440
53.140679	2394.123310	19.226458
53.499730	2386.772060	19.231475
53.205211	2374.544369	19.236493
53.307612	2371.041922	19.241511
53.351887	2365.813536	19.246528
53.298242	2360.109938	19.251546
53.588248	2361.426095	19.256563
53.308571	2368.533492	19.261581
53.497167	2367.281885	19.266599
53.527051	2360.485768	19.271616
53.320201	2361.806434	19.276634
53.096422	2360.485296	19.281651
53.185532	2368.510036	19.286669
53.617093	2392.755453	19.291687
53.982896	2393.626902	19.296704
53.625655	2401.395619	19.301722
54.153750	2399.927045	19.306739
54.055764	2406.052141	19.311757
54.015216	2395.264291	19.316775
54.017031	2374.414749	19.321792
53.619817	2378.784694	19.326810
53.920420	2383.728477	19.331827
53.821339	2396.431977	19.336845
54.100889	2395.142264	19.341863
54.093400	2408.070290	19.346880
53.867786	2411.987336	19.351898
53.956614	2392.148031	19.356915
53.838930	2399.827418	19.361933
54.071063	2410.106546	19.366951
54.239323	2419.986841	19.371968
54.408016	2431.672298	19.376986
54.600687	2425.477104	19.382003
54.265894	2439.826020	19.387021
54.271395	2444.142776	19.392039
54.449552	2436.567852	19.397056
54.050630	2442.294171	19.402074
54.564039	2450.778309	19.407091
54.574418	2467.386358	19.412109
54.547394	2461.939623	19.417127
54.725220	2465.937078	19.422144
54.739017	2467.525404	19.427162
54.659005	2464.867721	19.432179
54.621059	2468.589670	19.437197
54.818851	2485.389671	19.442215
55.442956	2488.530158	19.447232
55.286482	2493.474503	19.452250
55.249033	2490.291662	19.457267
55.620927	2491.782769	19.462285
55.514754	2489.398268	19.467303
55.883692	2487.988103	19.472320
55.834490	2492.772967	19.477338
55.894648	2485.622718	19.482355
55.934426	2488.439494	19.487373
55.772135	2476.364468	19.492391
55.757902	2481.059586	19.497408
55.300446	2473.369692	19.502426
55.737282	2473.639874	19.507443
56.184101	2478.469914	19.512461
56.057316	2483.943617	19.517479
56.068083	2475.362571	19.522496
55.612359	2478.576933	19.527514
56.144554	2474.598468	19.532531
55.918480	2479.208592	19.537549
55.956105	2480.366000	19.542567
56.256534	2475.740158	19.547584
55.995585	2485.216989	19.552602
55.851501	2482.458610	19.557619
56.316432	2507.820578	19.562637
56.183667	2512.514158	19.567655
56.621934	2506.930278	19.572672
56.528780	2508.191922	19.577690
56.596268	2502.237692	19.582707
56.629797	2510.832216	19.587725
56.579003	2518.028254	19.592743
56.985440	2505.319758	19.597760
56.297287	2516.264872	19.602778
56.711030	2513.397079	19.607795
56.707087	2516.032837	19.612813
56.731504	2512.601001	19.617831
57.121374	2521.304676	19.622848
56.652828	2536.561508	19.627866
56.976272	2536.430520	19.632883
57.012551	2537.168891	19.637901
57.342688	2542.889108	19.642919
57.498375	2533.692611	19.647936
57.323844	2542.619238	19.652954
57.287554	2537.680521	19.657971
57.611859	2537.477028	19.662989
57.192237	2530.268759	19.668007
57.439254	2527.846021	19.673024
57.026510	2548.349996	19.678042
57.316519	2557.056246	19.683059
57.730069	2570.476543	19.688077
57.622685	2578.535880	19.693095
57.741378	2565.116512	19.698112
57.480984	2574.975597	19.703130
57.667744	2569.133682	19.708147
58.138572	2573.270867	19.713165
57.840776	2594.285169	19.718183
58.568154	2593.509255	19.723200
58.333897	2605.589481	19.728218
58.340109	2592.838543	19.733235
58.539699	2594.622222	19.738253
58.340051	2601.009816	19.743271
58.651509	2584.602078	19.748288
58.473229	2599.207005	19.753306
58.422848	2598.396227	19.758323
58.708659	2596.244174	19.763341
58.535900	2598.795170	19.768359
58.512053	2593.453284	19.773376
58.784530	2604.124922	19.778394
58.889362	2595.715228	19.783411
59.092181	2593.837561	19.788429
58.856744	2590.483329	19.793447
59.114107	2584.690717	19.798464
59.062578	2588.078984	19.803482
58.804029	2592.680164	19.808499
58.994637	2585.930680	19.813517
59.081228	2587.938467	19.818535
59.075900	2586.520329	19.823552
58.607178	2594.652243	19.828570
58.789279	2608.173198	19.833587
59.158543	2612.433568	19.838605
58.990224	2627.937592	19.843623
59.481257	2618.689138	19.848640
59.302357	2621.932539	19.853658
59.436642	2626.713357	19.858675
59.291104	2637.223565	19.863693
59.308725	2645.320426	19.868711
59.694997	2654.567511	19.873728
59.594052	2656.558017	19.878746
59.466709	2648.110591	19.883763
59.922643	2655.140936	19.888781
59.887229	2652.563419	19.893799
60.386985	2655.936944	19.898816
60.256112	2652.836614	19.903834
60.225346	2654.287332	19.908851
60.372668	2644.237849	19.913869
60.240587	2644.198381	19.918887
60.688526	2664.577066	19.923904
60.715567	2651.019634	19.928922
60.596639	2638.431773	19.933939
60.932560	2635.402529	19.938957
60.945035	2636.535642	19.943975
60.886491	2621.026170	19.948992
61.105477	2627.871680	19.954010
60.749090	2630.628163	19.959027
60.872898	2629.143806	19.964045
60.978524	2633.066296	19.969063
61.519228	2624.838790	19.974080
61.240069	2628.675546	19.979098
61.258610	2626.768266	19.984115
61.781790	2616.800453	19.989133
61.497937	2627.748036	19.994151
61.680358	2623.568092	19.999168
61.701916	2615.859155	20.004186
61.496775	2605.959511	20.009203
61.576369	2587.817321	20.014221
61.506357	2579.842977	20.019239
61.461673	2590.079851	20.024256
61.631817	2614.342155	20.029274
61.513476	2623.006586	20.034291
61.744298	2608.228930	20.039309
61.807133	2609.328839	20.044327
61.908222	2609.053177	20.049344
62.064541	2606.288560	20.054362
61.629094	2620.575043	20.059379
61.756526	2612.370972	20.064397
61.651812	2618.840187	20.069415
61.614250	2609.674459	20.074432
61.807154	2631.437281	20.079450
61.948765	2652.186519	20.084467
62.222448	2648.740072	20.089485
62.085778	2651.960227	20.094503
61.932031	2651.531699	20.099520
62.218838	2645.422086	20.104538
62.050668	2649.622650	20.109555
62.410496	2663.273422	20.114573
62.553672	2676.732214	20.119591
62.652611	2674.795589	20.124608
62.214615	2676.949184	20.129626
62.117065	2684.864636	20.134643
62.761186	2682.334497	20.139661
62.866944	2687.288218	20.144679
62.406466	2698.901956	20.149696
62.449244	2713.168903	20.154714
62.552894	2710.245118	20.159731
62.605425	2717.114068	20.164749
62.940282	2719.395351	20.169767
63.382505	2731.227002	20.174784
63.762108	2740.754451	20.179802
63.663739	2741.297987	20.184819
63.719769	2729.335818	20.189837
63.357074	2733.027027	20.194855
63.301047	2737.077582	20.199872
63.794448	2730.415043	20.204890
63.479061	2735.008812	20.209907
63.902561	2735.843552	20.214925
63.643509	2741.192920	20.219943
63.530565	2733.065658	20.224960
64.040622	2727.003004	20.229978
63.932246	2730.407449	20.234995
64.048921	2733.584075	20.240013
64.041417	2726.852747	20.245031
64.242556	2755.826046	20.250048
64.542496	2753.199753	20.255066
64.601360	2764.007832	20.260083
64.474076	2749.311525	20.265101
64.286466	2748.519476	20.270119
64.490896	2746.672997	20.275136
64.818034	2752.046096	20.280154
64.675893	2766.012208	20.285171
64.816197	2748.149611	20.290189
64.663432	2757.299440	20.295207
64.454394	2761.909296	20.300224
65.037196	2756.347898	20.305242
64.845308	2770.646817	20.310259
65.071469	2759.250595	20.315277
64.795293	2759.786303	20.320295
64.559245	2753.652259	20.325312
65.076721	2762.187062	20.330330
64.843463	2781.349106	20.335347
65.108660	2778.467195	20.340365
65.262535	2786.792548	20.345383
65.205361	2790.117260	20.350400
65.504989	2785.505610	20.355418
65.087106	2789.156077	20.360435
65.465605	2785.602424	20.365453
65.701323	2811.393992	20.370471
65.754988	2815.319311	20.375488
66.047009	2816.084563	20.380506
65.736412	2825.714265	20.385523
65.977625	2814.887467	20.390541
65.987146	2819.265048	20.395559
65.743487	2819.738150	20.400576
65.815412	2813.218300	20.405594
65.927169	2818.927828	20.410611
66.078188	2813.127700	20.415629
65.972930	2810.574665	20.420647
66.109073	2821.164371	20.425664
66.356755	2832.522123	20.430682
66.259352	2850.051611	20.435699
66.756488	2846.360247	20.440717
66.441465	2855.311828	20.445735
66.392869	2856.710346	20.450752
66.390319	2849.854673	20.455770
66.264545	2852.550823	20.460787
66.652320	2857.090708	20.465805
66.770489	2881.381408	20.470823
67.053208	2883.942414	20.475840
67.144938	2881.862174	20.480858
67.168498	2880.961714	20.485875
67.258435	2875.447403	20.490893
67.427707	2871.518056	20.495911
67.329376	2876.922078	20.500928
67.373422	2873.277002	20.505946
67.525924	2866.463458	20.510963
67.629766	2873.096181	20.515981
67.734241	2868.927810	20.520999
67.396054	2867.456533	20.526016
67.552840	2860.302491	20.531034
67.353407	2877.414858	20.536051
67.665004	2880.510876	20.541069
67.839961	2885.192474	20.546087
67.796346	2899.957934	20.551104
67.950407	2893.243242	20.556122
68.010017	2901.693033	20.561139
68.051032	2895.259883	20.566157
67.994486	2896.402450	20.571175
68.569707	2894.970367	20.576192
68.747683	2886.468608	20.581210
68.326862	2887.172909	20.586227
68.629834	2895.958317	20.591245
68.892093	2888.929033	20.596263
68.474937	2891.460843	20.601280
68.635376	2880.003427	20.606298
68.737564	2895.295475	20.611315
68.722789	2895.888616	20.616333
68.906802	2908.995000	20.621351
68.872619	2927.922542	20.626368
68.774310	2918.528749	20.631386
69.084129	2935.395574	20.636403
69.364802	2920.150271	20.641421
69.877427	2895.467943	20.646439
70.042379	2882.096758	20.651456
69.953456	2873.241901	20.656474
69.910535	2866.041041	20.661491
70.022984	2859.636633	20.666509
70.072472	2866.200933	20.671527
69.773531	2860.615702	20.676544
70.140437	2853.733363	20.681562
70.345601	2854.478643	20.686579
69.871964	2846.624367	20.691597
70.081991	2828.929900	20.696615
69.870455	2826.238848	20.701632
69.944609	2826.186156	20.706650
69.726665	2844.276835	20.711667
69.880683	2854.853489	20.716685
70.037010	2853.319087	20.721703
70.132525	2870.111458	20.726720
70.436466	2856.522266	20.731738
70.094611	2855.675358	20.736755
70.158853	2865.721214	20.741773
70.334724	2857.950571	20.746791
70.291517	2884.399519	20.751808
70.506251	2885.408365	20.756826
70.442412	2884.067178	20.761843
70.461311	2888.999421	20.766861
70.670744	2888.199112	20.771879
70.411060	2893.255228	20.776896
70.996335	2902.440847	20.781914
70.584392	2929.050936	20.786931
70.850413	2921.247006	20.791949
71.033169	2916.580010	20.796967
70.804652	2932.233973	20.801984
71.147854	2942.815921	20.807002
71.128335	2950.597147	20.812019
71.509656	2955.095616	20.817037
71.840459	2953.711944	20.822055
71.591446	2958.588605	20.827072
71.799704	2947.269822	20.832090
71.483493	2944.470367	20.837107
71.504096	2960.354445	20.842125
71.937673	2949.651836	20.847143
71.836365	2959.560539	20.852160
71.988325	2941.273434	20.857178
71.529575	2955.141543	20.862195
71.628604	2970.302808	20.867213
71.839206	2970.193746	20.872231
71.858254	2973.670749	20.877248
72.279490	2989.049678	20.882266
72.537179	3006.178976	20.887283
72.139051	2998.316509	20.892301
72.722497	3002.903900	20.897319
72.588451	3005.823224	20.902336
72.823019	3007.543954	20.907354
72.852218	3003.021771	20.912371
72.778813	3003.869691	20.917389
72.958913	2995.848156	20.922407
72.718818	3008.124725	20.927424
73.170432	3003.316502	20.932442
73.161237	3001.606318	20.937459
72.965138	3007.505031	20.942477
73.394648	3012.813920	20.947495
73.204367	3023.429080	20.952512
73.213844	3026.645676	20.957530
73.497703	3029.960898	20.962547
73.541491	3039.012697	20.967565
73.731783	3034.004642	20.972583
73.005641	3049.476924	20.977600
73.533850	3039.340475	20.982618
73.730531	3030.803399	20.987635
73.696262	3048.629053	20.992653
74.036222	3065.366936	20.997671
73.981755	3070.735716	21.002688
74.068420	3076.337647	21.007706
73.951470	3074.265484	21.012723
73.876249	3075.403963	21.017741
74.164152	3065.212208	21.022759
73.965423	3070.171349	21.027776
74.094289	3080.727006	21.032794
74.420540	3085.019549	21.037811
74.350363	3098.198102	21.042829
74.673472	3086.337791	21.047847
74.522801	3092.297730	21.052864
74.608846	3097.607929	21.057882
74.700111	3088.858722	21.062899
75.033372	3112.058282	21.067917
75.276917	3112.485952	21.072935
75.424112	3119.878049	21.077952
75.331459	3111.748126	21.082970
75.808991	3119.356572	21.087987
75.267465	3120.831359	21.093005
75.516884	3100.056933	21.098023
75.608645	3113.931013	21.103040
75.293246	3119.730801	21.108058
75.332876	3119.090497	21.113075
75.361064	3119.792430	21.118093
75.753175	3116.572419	21.123111
75.455021	3133.150974	21.128128
75.341787	3127.908102	21.133146
75.850021	3141.900655	21.138163
75.674633	3153.321401	21.143181
75.907178	3158.115045	21.148199
75.852962	3145.879063	21.153216
76.031551	3163.529321	21.158234
76.645551	3169.830680	21.163251
76.648826	3175.062070	21.168269
76.944494	3174.028525	21.173287
77.014696	3179.970585	21.178304
76.871912	3148.141190	21.183322
76.978343	3142.250501	21.188339
76.732212	3150.129326	21.193357
76.345931	3146.442675	21.198375
76.896687	3158.759237	21.203392
76.779883	3173.686891	21.208410
77.251070	3174.922317	21.213427
77.035876	3180.216078	21.218445
77.162538	3181.813230	21.223463
77.123497	3178.572282	21.228480
77.112654	3175.667450	21.233498
76.899005	3177.390450	21.238515
76.941992	3187.657813	21.243533
77.318127	3198.809723	21.248551
77.426041	3204.206150	21.253568
77.330207	3203.353814	21.258586
77.560063	3199.922883	21.263603
77.887303	3222.415610	21.268621
78.238788	3224.167281	21.273639
77.925683	3237.554609	21.278656
78.187529	3226.256172	21.283674
78.341223	3223.805726	21.288691
78.279090	3233.406299	21.293709
78.263825	3231.050444	21.298727
78.736028	3223.371590	21.303744
78.216378	3226.132189	21.308762
78.667813	3232.695488	21.313779
78.089482	3228.402267	21.318797
78.345108	3226.529474	21.323815
78.518649	3256.754194	21.328832
78.799931	3260.300364	21.333850
78.846611	3245.288696	21.338867
78.714537	3252.592451	21.343885
79.100248	3259.085220	21.348903
79.033457	3252.366251	21.353920
79.016174	3260.449352	21.358938
79.170376	3281.837010	21.363955
79.276890	3289.356822	21.368973
79.563473	3279.953339	21.373991
79.330379	3282.835020	21.379008
79.357146	3290.612193	21.384026
79.819358	3285.775443	21.389043
79.673295	3299.509843	21.394061
79.869857	3291.166149	21.399079
79.849704	3302.367171	21.404096
80.386587	3317.269396	21.409114
80.149962	3311.965897	21.414131
80.359119	3325.141016	21.419149
80.453195	3314.597691	21.424167
80.684560	3312.580868	21.429184
80.597067	3308.929126	21.434202
80.802945	3301.237636	21.439219
80.598309	3312.671823	21.444237
81.051096	3301.206006	21.449255
80.873975	3304.169229	21.454272
80.674601	3302.709595	21.459290
80.769590	3303.087803	21.464307
80.768063	3318.055432	21.469325
81.222968	3308.302569	21.474343
81.066969	3302.639309	21.479360
80.640059	3311.280193	21.484378
80.751654	3302.490644	21.489395
80.988229	3327.029087	21.494413
81.062637	3337.674637	21.499431
81.513300	3342.962969	21.504448
81.530248	3348.394407	21.509466
81.607750	3329.745825	21.514483
81.563525	3345.429838	21.519501
81.619895	3334.192403	21.524519
81.735028	3331.117203	21.529536
81.464259	3365.239206	21.534554
82.003031	3356.374428	21.539571
81.955104	3375.207983	21.544589
82.045957	3364.628164	21.549607
82.495828	3364.970238	21.554624
82.341979	3375.732450	21.559642
82.655021	3368.080475	21.564659
82.497437	3373.428050	21.569677
82.303790	3368.209714	21.574695
82.473247	3366.489092	21.579712
82.362858	3396.298404	21.584730
82.837077	3386.818522	21.589747
82.899996	3385.343799	21.594765
82.848391	3387.603433	21.599783
83.209711	3390.468227	21.604800
82.929695	3388.152991	21.609818
83.198445	3386.094798	21.614835
83.098909	3393.305330	21.619853
83.115407	3410.491656	21.624871
83.582558	3414.185220	21.629888
83.372050	3414.825326	21.634906
83.422306	3415.312935	21.639923
83.313914	3418.717540	21.644941
83.557736	3419.979806	21.649959
84.078058	3429.239837	21.654976
83.968875	3441.223713	21.659994
84.109856	3438.359910	21.665011
84.340246	3441.520918	21.670029
84.509740	3439.749151	21.675047
84.996742	3435.519624	21.680064
84.555600	3431.254023	21.685082
84.838103	3407.133012	21.690099
84.783022	3396.201212	21.695117
84.819632	3390.297171	21.700135
84.805551	3387.376294	21.705152
84.730479	3393.200010	21.710170
85.430156	3416.163845	21.715187
85.346600	3406.543192	21.720205
85.049297	3394.732006	21.725223
85.218110	3396.454616	21.730240
84.870150	3399.878539	21.735258
84.941355	3422.763245	21.740275
85.428925	3423.827741	21.745293
85.326455	3423.178618	21.750311
85.250151	3428.407842	21.755328
85.386133	3430.658809	21.760346
85.644504	3427.108429	21.765363
85.545882	3425.550905	21.770381
85.431394	3436.959014	21.775399
85.598397	3451.267443	21.780416
85.604682	3460.551251	21.785434
85.738050	3461.842145	21.790451
85.632037	3461.638826	21.795469
85.796922	3475.466190	21.800487
86.092306	3481.046794	21.805504
86.014453	3492.313014	21.810522
86.406033	3491.177624	21.815539
86.343343	3488.081975	21.820557
86.190495	3496.090852	21.825575
86.829447	3501.569480	21.830592
86.784426	3512.306573	21.835610
87.302600	3497.771691	21.840627
87.570926	3506.212149	21.845645
87.310325	3511.377966	21.850663
87.617190	3504.488380	21.855680
87.231135	3501.643314	21.860698
87.232621	3496.050837	21.865715
87.229917	3501.730113	21.870733
87.130738	3499.783279	21.875751
87.743663	3495.488030	21.880768
87.238032	3507.712959	21.885786
87.472708	3513.001183	21.890803
87.489449	3529.821031	21.895821
87.672331	3537.299687	21.900839
87.946945	3537.444731	21.905856
87.698850	3553.189794	21.910874
88.007639	3532.314826	21.915891
88.448469	3550.076345	21.920909
88.114838	3555.154704	21.925927
88.203854	3552.285006	21.930944
88.203529	3565.433173	21.935962
88.147233	3556.339851	21.940979
88.436797	3554.751880	21.945997
88.518041	3587.037291	21.951015
88.627553	3581.414970	21.956032
88.866958	3589.384164	21.961050
88.923926	3582.166237	21.966067
89.175645	3589.934444	21.971085
88.871534	3593.347486	21.976103
89.357305	3594.698625	21.981120
89.636607	3606.201403	21.986138
89.844465	3610.295079	21.991155
89.685224	3607.067696	21.996173
89.950866	3606.046778	22.001191
89.943252	3603.169666	22.006208
89.756929	3615.136091	22.011226
90.011329	3606.541493	22.016243
90.318271	3605.697279	22.021261
89.771003	3608.400204	22.026279
89.864091	3604.286147	22.031296
89.793914	3605.149320	22.036314
89.793918	3605.494697	22.041331
90.162657	3616.834545	22.046349
90.125673	3644.923258	22.051367
90.387287	3632.780466	22.056384
90.387463	3645.169504	22.061402
90.702301	3639.747270	22.066419
90.877778	3631.383146	22.071437
90.632893	3639.796171	22.076455
90.983885	3652.189847	22.081472
91.118769	3656.115028	22.086490
91.019088	3664.767657	22.091507
91.215992	3658.391915	22.096525
90.998306	3674.809569	22.101543
91.699834	3660.569393	22.106560
91.545882	3657.937441	22.111578
91.655640	3661.789538	22.116595
91.970115	3655.689259	22.121613
91.666306	3658.634207	22.126631
92.009338	3668.328577	22.131648
91.968061	3686.925474	22.136666
92.142644	3687.301228	22.141683
92.085170	3689.833240	22.146701
92.086793	3696.338679	22.151719
92.917553	3693.016349	22.156736
92.585813	3698.902353	22.161754
92.424297	3692.965277	22.166771
92.745040	3687.215621	22.171789
92.460117	3699.685565	22.176807
92.599697	3687.884717	22.181824
92.402709	3693.857003	22.186842
92.787785	3719.829317	22.191859
92.947862	3716.347248	22.196877
92.767641	3723.983804	22.201895
93.073577	3725.904854	22.206912
93.250092	3735.659647	22.211930
93.322332	3744.680599	22.216947
93.637496	3743.695829	22.221965
93.470575	3754.557948	22.226983
93.769778	3744.535416	22.232000
93.849953	3739.071899	22.237018
93.809816	3733.791979	22.242035
94.035022	3737.449476	22.247053
93.987414	3739.797418	22.252071
94.333329	3751.284969	22.257088
94.174214	3761.393015	22.262106
94.638795	3762.888362	22.267123
94.860269	3763.589399	22.272141
94.755801	3777.030481	22.277159
94.892603	3764.519658	22.282176
95.037810	3763.884519	22.287194
94.863700	3778.253167	22.292211
94.893065	3763.643354	22.297229
94.621340	3773.337487	22.302247
94.780864	3762.081703	22.307264
94.817314	3768.729512	22.312282
94.817878	3765.765318	22.317299
95.080790	3779.970670	22.322317
95.087232	3803.784332	22.327335
95.305699	3804.121626	22.332352
95.378436	3803.775732	22.337370
95.052041	3805.246956	22.342387
95.237140	3814.305022	22.347405
95.467964	3829.143296	22.352423
95.532394	3826.618878	22.357440
95.825021	3835.180732	22.362458
95.954150	3855.213868	22.367475
96.330200	3857.964702	22.372493
96.273724	3866.365907	22.377511
96.399645	3861.730490	22.382528
96.743416	3859.249631	22.387546
96.155497	3861.979534	22.392563
96.444273	3860.380644	22.397581
96.531731	3880.800420	22.402599
96.662949	3885.365021	22.407616
97.100653	3893.143855	22.412634
96.867958	3896.603791	22.417651
96.939237	3888.626657	22.422669
97.120879	3890.622615	22.427687
97.201055	3911.001114	22.432704
97.392523	3922.718747	22.437722
96.946661	3926.771216	22.442739
97.224709	3922.972927	22.447757
97.524168	3931.032639	22.452775
98.255128	3930.083039	22.457792
98.420243	3931.282380	22.462810
98.195288	3932.856228	22.467827
98.399172	3925.764174	22.472845
98.375711	3938.282308	22.477863
98.254571	3935.143965	22.482880
98.653653	3921.464675	22.487898
98.690111	3931.794174	22.492915
98.680423	3923.443676	22.497933
98.398373	3929.082699	22.502951
98.774391	3926.970356	22.507968
98.800095	3936.365435	22.512986
98.535322	3945.358434	22.518003
98.915378	3958.046671	22.523021
98.944267	3961.385458	22.528039
99.006072	3961.611642	22.533056
99.301900	3964.103887	22.538074
99.349428	3989.652205	22.543091
99.437341	3990.927582	22.548109
99.335387	4011.628691	22.553127
99.619576	4009.608859	22.558144
99.571535	3999.075119	22.563162
99.523586	4010.549369	22.568179
99.925765	4024.177359	22.573197
99.947107	4027.877662	22.578215
99.929705	4033.676702	22.583232
100.307821	4037.006235	22.588250
100.000827	4041.057045	22.593267
100.328139	4045.070436	22.598285
100.369672	4048.940594	22.603303
100.540737	4062.046143	22.608320
100.889916	4052.618816	22.613338
100.620458	4058.858475	22.618355
100.853741	4068.754694	22.623373
101.141698	4085.641281	22.628391
101.074301	4090.897640	22.633408
101.301659	4099.927904	22.638426
101.171005	4103.816091	22.643443
101.397791	4090.332469	22.648461
101.285877	4085.515421	22.653479
101.260806	4099.243075	22.658496
101.757507	4103.792735	22.663514
101.692773	4123.471676	22.668531
101.790035	4117.965959	22.673549
102.144092	4119.610345	22.678567
101.846866	4121.159548	22.683584
102.173018	4139.243729	22.688602
102.268575	4152.318918	22.693619
102.384846	4157.391038	22.698637
102.438996	4159.374322	22.703655
102.474004	4157.134598	22.708672
102.878821	4158.165149	22.713690
102.950266	4175.781790	22.718707
103.035296	4182.659619	22.723725
103.458209	4184.577813	22.728743
103.195035	4187.442436	22.733760
103.514510	4176.269395	22.738778
103.403278	4187.645311	22.743795
103.319541	4175.818320	22.748813
103.414567	4181.087360	22.753831
103.678764	4174.914644	22.758848
103.957941	4182.963569	22.763866
103.690191	4202.602611	22.768883
103.832608	4207.440081	22.773901
103.979381	4211.828447	22.778919
103.898600	4209.059645	22.783936
104.755610	4205.454535	22.788954
104.414343	4217.118106	22.793971
104.412868	4208.629254	22.798989
104.258997	4230.462334	22.804007
104.639207	4247.866199	22.809024
104.978439	4244.910842	22.814042
104.435968	4241.484031	22.819059
104.597542	4241.905930	22.824077
105.361109	4262.985451	22.829095
105.147350	4268.498070	22.834112
105.570475	4271.335094	22.839130
105.438158	4285.120929	22.844147
105.566691	4276.541292	22.849165
105.640616	4271.943145	22.854183
105.467145	4280.402575	22.859200
105.838991	4283.412196	22.864218
105.737541	4292.268441	22.869235
106.085119	4300.052423	22.874253
106.305066	4314.173102	22.879271
106.339098	4320.797159	22.884288
106.438691	4312.996220	22.889306
106.301311	4322.146927	22.894323
106.286588	4302.965066	22.899341
106.451188	4311.113361	22.904359
106.378913	4306.528288	22.909376
106.910072	4324.118221	22.914394
106.913562	4342.562483	22.919411
106.838890	4348.992266	22.924429
107.352460	4344.012466	22.929447
107.211667	4339.873348	22.934464
107.486796	4334.377739	22.939482
107.091329	4342.010386	22.944499
107.358892	4350.439655	22.949517
107.573533	4363.986941	22.954535
107.611411	4374.630415	22.959552
107.742841	4367.815606	22.964570
107.677989	4366.749786	22.969587
108.003495	4375.991139	22.974605
108.187248	4388.347598	22.979623
108.177728	4400.661721	22.984640
108.357233	4393.613453	22.989658
108.370258	4402.532540	22.994675
108.754791	4397.407304	22.999693
108.660903	4391.110655	23.004711
108.795797	4411.046079	23.009728
109.387077	4411.394748	23.014746
109.211677	4417.846128	23.019763
109.287576	4410.261324	23.024781
109.323738	4413.659629	23.029799
109.422033	4413.983060	23.034816
109.206147	4419.016189	23.039834
109.382919	4418.571877	23.044851
109.480124	4435.313063	23.049869
109.667394	4438.652666	23.054887
109.571013	4457.051633	23.059904
109.765616	4456.665053	23.064922
109.692620	4464.245559	23.069939
109.894558	4482.279165	23.074957
110.117806	4476.640730	23.079975
109.858598	4488.242654	23.084992
110.057447	4497.420888	23.090010
110.357529	4510.733624	23.095027
110.631441	4513.244406	23.100045
110.783493	4510.878188	23.105063
110.550468	4525.877664	23.110080
110.613992	4537.045044	23.115098
110.816122	4554.789202	23.120115
110.888318	4541.741263	23.125133
111.529544	4567.339887	23.130151
111.524320	4582.989892	23.135168
111.626951	4571.823594	23.140186
111.670900	4575.730480	23.145203
111.991736	4568.680048	23.150221
111.875202	4573.309542	23.155239
111.799940	4565.862046	23.160256
111.886726	4581.163816	23.165274
112.226534	4582.288156	23.170291
112.310905	4592.634866	23.175309
112.783479	4591.962443	23.180327
113.105538	4600.291909	23.185344
113.252426	4589.754986	23.190362
113.104517	4589.004488	23.195379
113.255720	4592.849435	23.200397
113.344815	4592.348295	23.205415
113.086842	4594.686647	23.210432
113.218794	4589.550483	23.215450
113.335547	4593.907562	23.220467
113.363811	4599.429703	23.225485
113.158266	4587.554932	23.230503
113.462285	4618.295825	23.235520
114.080897	4615.414643	23.240538
113.777870	4628.173829	23.245555
113.784563	4636.843108	23.250573
113.949238	4625.201932	23.255591
113.989376	4639.806310	23.260608
114.256666	4638.825186	23.265626
114.314238	4650.398755	23.270643
114.477871	4648.951118	23.275661
114.645907	4649.445951	23.280679
114.488716	4670.140269	23.285696
114.757600	4682.743803	23.290714
115.070580	4687.607733	23.295731
114.805926	4680.372893	23.300749
115.252296	4673.882988	23.305767
115.559749	4693.275199	23.310784
115.637589	4713.521441	23.315802
115.865644	4706.766594	23.320819
115.571281	4710.084714	23.325837
116.028652	4715.234022	23.330855
116.048595	4712.444344	23.335872
116.302963	4703.972630	23.340890
115.928086	4697.597924	23.345907
115.922957	4714.335289	23.350925
116.471176	4723.365915	23.355943
116.403075	4725.986337	23.360960
116.205203	4735.706298	23.365978
116.555666	4726.855787	23.370995
116.565118	4751.037110	23.376013
116.703748	4765.323810	23.381031
117.137293	4765.969058	23.386048
117.145343	4771.352091	23.391066
117.074392	4767.214304	23.396083
117.209987	4783.639798	23.401101
117.789978	4785.152260	23.406119
117.919812	4795.539067	23.411136
117.735623	4801.753641	23.416154
118.105047	4792.487041	23.421171
117.838246	4798.340308	23.426189
118.461065	4797.731247	23.431207
118.466402	4796.149919	23.436224
118.178393	4795.984251	23.441242
118.178911	4790.628239	23.446259
118.138610	4815.120485	23.451277
118.382376	4806.719634	23.456295
118.359236	4831.055761	23.461312
118.319439	4826.478721	23.466330
118.606380	4849.887460	23.471347
118.602823	4856.859189	23.476365
118.941004	4864.165072	23.481383
119.122244	4868.047786	23.486400
118.828827	4884.688126	23.491418
119.306034	4886.877046	23.496435
119.321556	4893.247842	23.501453
119.939500	4897.573089	23.506471
119.682088	4916.271297	23.511488
119.707753	4907.272638	23.516506
119.882548	4924.613292	23.521523
119.846207	4928.337966	23.526541
120.139658	4940.656944	23.531559
120.393662	4948.748855	23.536576
120.415041	4945.013261	23.541594
120.502259	4969.516113	23.546611
120.433880	4981.169028	23.551629
120.999024	4971.968666	23.556647
121.168708	4972.442792	23.561664
121.128642	4978.117580	23.566682
121.651493	4986.235091	23.571699
121.397531	5002.162005	23.576717
121.561815	5005.895620	23.581735
121.626413	5010.519972	23.586752
121.596184	5006.212773	23.591770
122.121110	5001.344236	23.596787
121.888282	5024.631577	23.601805
122.045664	5032.669707	23.606823
122.212499	5030.077619	23.611840
122.147539	5032.856514	23.616858
122.538801	5037.287966	23.621875
122.983741	5051.463954	23.626893
123.110048	5045.050883	23.631911
123.297270	5050.954588	23.636928
123.374402	5057.512313	23.641946
123.524092	5047.670874	23.646963
123.504709	5058.928181	23.651981
123.592072	5041.369416	23.656999
123.463727	5052.803797	23.662016
123.815978	5047.427801	23.667034
124.094350	5039.531102	23.672051
123.902568	5053.545058	23.677069
124.139106	5047.496761	23.682087
124.217721	5057.961152	23.687104
124.246817	5051.149758	23.692122
124.165784	5062.281579	23.697139
124.261292	5088.997169	23.702157
124.503858	5076.277198	23.707175
124.330099	5078.982187	23.712192
124.218351	5086.191559	23.717210
124.894572	5095.790483	23.722227
124.593551	5107.934536	23.727245
124.839894	5111.647227	23.732263
124.974968	5121.490583	23.737280
125.216814	5132.018690	23.742298
125.786830	5131.467603	23.747315
125.601541	5139.331488	23.752333
125.539432	5140.250106	23.757351
125.819963	5147.549589	23.762368
125.735955	5159.495442	23.767386
125.904961	5170.850248	23.772403
126.062623	5174.780073	23.777421
126.304853	5182.266630	23.782439
126.654270	5198.425620	23.787456
126.718346	5205.077541	23.792474
126.883958	5195.731471	23.797491
126.741467	5203.978789	23.802509
127.149704	5201.172740	23.807527
127.082213	5202.860077	23.812544
126.980238	5216.179339	23.817562
127.308982	5227.972896	23.822579
127.682283	5237.487253	23.827597
127.757448	5228.567835	23.832615
127.975949	5224.013215	23.837632
127.556547	5235.818280	23.842650
128.097469	5237.518759	23.847667
128.308808	5259.815166	23.852685
128.389941	5259.085546	23.857703
128.189330	5249.542928	23.862720
128.076209	5248.981173	23.867738
128.506535	5260.713717	23.872755
128.637851	5276.256932	23.877773
129.025552	5277.498786	23.882791
128.679035	5277.329850	23.887808
128.992795	5292.139859	23.892826
129.213760	5303.546276	23.897843
129.420090	5323.589557	23.902861
129.849925	5318.842290	23.907879
130.627351	5300.687773	23.912896
130.636327	5302.207941	23.917914
130.774638	5299.771410	23.922931
131.144485	5304.688633	23.927949
130.805960	5297.325225	23.932967
130.939540	5286.056683	23.937984
130.671291	5276.834809	23.943002
130.988993	5273.371303	23.948019
131.018286	5294.571747	23.953037
130.784513	5300.806235	23.958055
130.784741	5287.274251	23.963072
130.731464	5300.653485	23.968090
130.890527	5290.160541	23.973107
130.925708	5286.439968	23.978125
131.159238	5307.122446	23.983143
131.486058	5313.229795	23.988160
131.103187	5323.824600	23.993178
131.705500	5327.302787	23.998195
131.335962	5337.387239	24.003213
131.601636	5351.216035	24.008231
132.081882	5343.947069	24.013248
132.455913	5372.069524	24.018266
132.494822	5372.547994	24.023283
132.904524	5371.241221	24.028301
132.500875	5382.541159	24.033319
132.846984	5376.660145	24.038336
132.664302	5386.714051	24.043354
133.213290	5404.532959	24.048371
133.303646	5409.526249	24.053389
133.143251	5405.504820	24.058407
133.225101	5409.846465	24.063424
133.081536	5417.248316	24.068442
133.448785	5429.803765	24.073459
133.675646	5438.443919	24.078477
133.771392	5441.424638	24.083495
134.118168	5460.386747	24.088512
134.171061	5475.370707	24.093530
134.456211	5469.546581	24.098547
134.400279	5469.715246	24.103565
134.558780	5485.927022	24.108583
134.835033	5482.507055	24.113600
134.759384	5495.318061	24.118618
134.590585	5497.871278	24.123635
134.913140	5507.994196	24.128653
135.131538	5515.920585	24.133671
135.273967	5523.253288	24.138688
135.077479	5527.141328	24.143706
135.292158	5539.473368	24.148723
135.610863	5548.046231	24.153741
135.506584	5567.309337	24.158759
135.946681	5569.198233	24.163776
135.993415	5592.285329	24.168794
136.107676	5581.986570	24.173811
136.726920	5599.234341	24.178829
136.811924	5607.416501	24.183847
137.033301	5604.680296	24.188864
136.838571	5613.286277	24.193882
137.089018	5605.893324	24.198899
137.378643	5611.759686	24.203917
137.047466	5633.858348	24.208935
137.518517	5638.090014	24.213952
137.445337	5647.157347	24.218970
137.691120	5639.446483	24.223987
137.980105	5656.132514	24.229005
138.272059	5675.707087	24.234023
138.758446	5676.402178	24.239040
138.522024	5681.706506	24.244058
138.690054	5690.875452	24.249075
138.920641	5687.729433	24.254093
138.598216	5684.252239	24.259111
138.906855	5687.162874	24.264128
139.118331	5682.201691	24.269146
138.997164	5688.892806	24.274163
139.153372	5686.432902	24.279181
138.926127	5704.910146	24.284199
139.574480	5711.307854	24.289216
139.058223	5711.025142	24.294234
139.330703	5733.028493	24.299251
139.829408	5731.068647	24.304269
139.847078	5748.959308	24.309287
140.106356	5730.654785	24.314304
140.024214	5752.068769	24.319322
140.097887	5762.652464	24.324339
140.921485	5775.564239	24.329357
140.765991	5772.718148	24.334375
141.149780	5776.248595	24.339392
140.758097	5776.765046	24.344410
140.918232	5792.976111	24.349427
141.222310	5790.498909	24.354445
140.837163	5804.498770	24.359463
141.282815	5816.461413	24.364480
141.314409	5823.103056	24.369498
141.534152	5829.008183	24.374515
141.721528	5844.567449	24.379533
141.546464	5862.754118	24.384551
141.723327	5858.545830	24.389568
141.950260	5880.637701	24.394586
142.236293	5888.271841	24.399603
142.620197	5894.095748	24.404621
142.303002	5909.760705	24.409639
142.967795	5915.893099	24.414656
143.152076	5926.296413	24.419674
142.911050	5928.716451	24.424691
143.321435	5942.426744	24.429709
143.182004	5962.014612	24.434727
143.560549	5958.728503	24.439744
143.427217	5962.919725	24.444762
143.461946	5994.353939	24.449779
144.154068	5987.398640	24.454797
144.231050	6000.358840	24.459815
145.066406	5993.033732	24.464832
145.376839	5995.712043	24.469850
145.214147	5987.761640	24.474867
145.374036	5966.195734	24.479885
145.341021	5972.254514	24.484903
145.480697	5970.235436	24.489920
145.918555	5982.953192	24.494938
145.977469	5983.900560	24.499955
146.034485	5966.797149	24.504973
145.548644	5977.013083	24.509991
146.066486	5985.484429	24.515008
145.841775	6000.105628	24.520026
145.898455	6013.053340	24.525043
146.083910	6005.682353	24.530061
145.965226	6007.370862	24.535079
146.320889	6026.458166	24.540096
146.234637	6039.323260	24.545114
146.018030	6044.126523	24.550131
146.640181	6052.118649	24.555149
146.549183	6074.636007	24.560167
146.626514	6080.914060	24.565184
146.784788	6085.184710	24.570202
146.870624	6101.965004	24.575219
146.826832	6114.506319	24.580237
147.435922	6138.599815	24.585255
147.894618	6133.296155	24.590272
148.200026	6154.676469	24.595290
148.016074	6164.161467	24.600307
148.760207	6152.296890	24.605325
149.021298	6154.659728	24.610343
149.055975	6149.246636	24.615360
149.464304	6147.637107	24.620378
149.398579	6152.786926	24.625395
149.479284	6147.800018	24.630413
149.458503	6155.018221	24.635431
149.610641	6145.202417	24.640448
149.560703	6152.282859	24.645466
149.554560	6173.020497	24.650483
150.340734	6168.866829	24.655501
150.245656	6179.097706	24.660519
149.808112	6185.048760	24.665536
150.048653	6185.315722	24.670554
150.214603	6203.813511	24.675571
150.459331	6208.814719	24.680589
150.504746	6219.139669	24.685607
150.827730	6222.517054	24.690624
150.998582	6237.281560	24.695642
150.740903	6253.833547	24.700659
151.205036	6240.309346	24.705677
151.329633	6270.994954	24.710695
151.239273	6275.306873	24.715712
151.674238	6276.435853	24.720730
151.756031	6294.422379	24.725747
151.842325	6305.590613	24.730765
151.562643	6309.931939	24.735783
152.371737	6326.464996	24.740800
152.054224	6335.189318	24.745818
152.299979	6341.103880	24.750835
152.553247	6347.944096	24.755853
152.551369	6363.451467	24.760871
152.644371	6370.610721	24.765888
153.288500	6373.663921	24.770906
153.633599	6386.629708	24.775923
154.004727	6378.624672	24.780941
153.886398	6393.305615	24.785959
154.127984	6383.383338	24.790976
154.018870	6390.256957	24.795994
153.753993	6398.010666	24.801011
153.935540	6403.963028	24.806029
154.028191	6415.349849	24.811047
154.396284	6432.872320	24.816064
154.753362	6431.385019	24.821082
154.934197	6449.498355	24.826099
155.071457	6456.078588	24.831117
155.012442	6458.444515	24.836135
155.167619	6456.343434	24.841152
155.467986	6470.617014	24.846170
155.490245	6477.867066	24.851187
155.576675	6487.601068	24.856205
155.617174	6499.221294	24.861223
155.590932	6523.330161	24.866240
156.086968	6527.970394	24.871258
155.729198	6533.662595	24.876275
156.088794	6550.525640	24.881293
156.263988	6569.802140	24.886311
156.774025	6587.701865	24.891328
157.118701	6579.165121	24.896346
156.802220	6587.540081	24.901363
157.413706	6601.920763	24.906381
157.503274	6615.520746	24.911399
157.936593	6621.636842	24.916416
157.590405	6624.545844	24.921434
157.862775	6629.544362	24.926451
158.357132	6642.896508	24.931469
158.049517	6658.761360	24.936487
158.341487	6658.685737	24.941504
158.710091	6642.214043	24.946522
158.874903	6673.533752	24.951539
159.169558	6675.546699	24.956557
159.009068	6681.467940	24.961575
158.917312	6691.582190	24.966592
159.242734	6697.452722	24.971610
159.390287	6706.910391	24.976627
159.341812	6724.080245	24.981645
159.585290	6727.309912	24.986663
159.542910	6747.553712	24.991680
160.288664	6748.103653	24.996698
159.926595	6766.448704	25.001715
160.224274	6778.657605	25.006733
160.378698	6772.783002	25.011751
160.644636	6781.379946	25.016768
160.939274	6794.505205	25.021786
160.843457	6813.231964	25.026803
161.241517	6803.845467	25.031821
161.117366	6826.108023	25.036839
161.186975	6835.482208	25.041856
161.604446	6837.314298	25.046874
161.699608	6862.140040	25.051891
161.867254	6871.936094	25.056909
161.778160	6871.857489	25.061927
161.986644	6877.640514	25.066944
162.510900	6888.803884	25.071962
162.437060	6902.545845	25.076979
162.679814	6899.493628	25.081997
163.013662	6919.696565	25.087015
163.044859	6933.103929	25.092032
163.529663	6933.876453	25.097050
163.248023	6939.915464	25.102067
163.259459	6937.712126	25.107085
163.937933	6957.750017	25.112103
163.928355	6957.839706	25.117120
163.935333	6953.773072	25.122138
164.223053	6984.777994	25.127155
164.695910	6998.733457	25.132173
164.718303	6993.472302	25.137191
164.643904	6994.517313	25.142208
164.746312	6998.520169	25.147226
165.112781	7011.163642	25.152243
165.028690	7023.199918	25.157261
165.166627	7025.077384	25.162279
164.836584	7039.198655	25.167296
165.617949	7043.703079	25.172314
165.353387	7065.716919	25.177331
165.905084	7071.026706	25.182349
165.810954	7079.805548	25.187367
165.719764	7098.904102	25.192384
166.226876	7122.523687	25.197402
166.336584	7130.240088	25.202419
166.613176	7151.030795	25.207437
167.070082	7151.002054	25.212455
167.184498	7155.280006	25.217472
167.676047	7171.710024	25.222490
167.707637	7186.986306	25.227507
167.854428	7190.228343	25.232525
167.801846	7193.918405	25.237543
167.930343	7196.560636	25.242560
168.243411	7215.029150	25.247578
168.292536	7219.742426	25.252595
168.380964	7225.231563	25.257613
168.637810	7230.393277	25.262631
168.701202	7241.807427	25.267648
169.053382	7256.419718	25.272666
169.263525	7259.706749	25.277683
169.547697	7267.789618	25.282701
169.660462	7278.267445	25.287719
169.680477	7282.764278	25.292736
169.973151	7276.736820	25.297754
170.106290	7287.123278	25.302771
170.316864	7302.072142	25.307789
170.255505	7294.435358	25.312807
170.347088	7308.689526	25.317824
170.550268	7324.992186	25.322842
170.414375	7342.872265	25.327859
170.756907	7340.099122	25.332877
171.285351	7358.513021	25.337895
171.070279	7374.472464	25.342912
171.370296	7378.253501	25.347930
171.472785	7382.141567	25.352947
171.818445	7401.720089	25.357965
171.999068	7410.342803	25.362983
171.897985	7408.719935	25.368000
172.220636	7410.220213	25.373018
172.323767	7437.761083	25.378035
172.454687	7433.045861	25.383053
172.757223	7440.401990	25.388071
172.673862	7451.325092	25.393088
172.746196	7446.730152	25.398106
173.039036	7458.929369	25.403123
173.104818	7485.192915	25.408141
173.397388	7484.259520	25.413159
173.775121	7502.035088	25.418176
174.166831	7506.024222	25.423194
174.080314	7508.184607	25.428211
174.008080	7512.096628	25.433229
174.418342	7537.224988	25.438247
174.342454	7541.748991	25.443264
174.568314	7560.634711	25.448282
174.965412	7571.237378	25.453299
174.968478	7578.024415	25.458317
175.592945	7593.797532	25.463335
175.731748	7599.305530	25.468352
176.264782	7598.484871	25.473370
176.323092	7600.368024	25.478387
176.004459	7607.010430	25.483405
176.469254	7616.009721	25.488423
176.481643	7628.371030	25.493440
176.706079	7627.257279	25.498458
176.847972	7642.860305	25.503475
176.998016	7653.500843	25.508493
177.442227	7667.837627	25.513511
177.248165	7669.185820	25.518528
177.421702	7678.707637	25.523546
177.911002	7693.680131	25.528563
177.941327	7703.489183	25.533581
178.181248	7698.617225	25.538599
177.985349	7716.291715	25.543616
178.168093	7732.795585	25.548634
178.468225	7729.039246	25.553651
178.188832	7750.094112	25.558669
178.755090	7750.661703	25.563687
178.830808	7770.496200	25.568704
179.301429	7778.071206	25.573722
179.417264	7792.529705	25.578739
179.139955	7800.573329	25.583757
179.663357	7814.367276	25.588775
179.711944	7823.596715	25.593792
180.021192	7840.509386	25.598810
180.262910	7852.620290	25.603827
180.337431	7863.188034	25.608845
180.960537	7872.444734	25.613863
180.957672	7894.375581	25.618880
180.945294	7891.317412	25.623898
181.131875	7902.014466	25.628915
181.388073	7897.114670	25.633933
181.521882	7910.199671	25.638951
181.535317	7925.902159	25.643968
181.543196	7919.239981	25.648986
182.001435	7934.509603	25.654003
181.804673	7958.407974	25.659021
182.467044	7953.741637	25.664039
182.611594	7966.559796	25.669056
182.678836	7990.620721	25.674074
183.146328	7985.721049	25.679092
183.191526	7993.930543	25.684109
183.765694	8009.635401	25.689127
183.395214	8018.465537	25.694144
183.304301	8021.120074	25.699162
183.755310	8022.727431	25.704180
183.627724	8045.240613	25.709197
183.844485	8057.005103	25.714215
184.147452	8067.443722	25.719232
184.466049	8081.288665	25.724250
184.523815	8092.620166	25.729268
184.558059	8110.040069	25.734285
185.130203	8120.200925	25.739303
185.521262	8144.929698	25.744320
185.347518	8161.033686	25.749338
185.881323	8150.485288	25.754356
185.588583	8167.113046	25.759373
185.689914	8182.623954	25.764391
185.815532	8209.357273	25.769408
186.188130	8215.268891	25.774426
186.423897	8225.333540	25.779444
186.333929	8240.098728	25.784461
187.098717	8240.362426	25.789479
186.792685	8248.804317	25.794496
187.374962	8264.561662	25.799514
187.684942	8265.616698	25.804532
187.741898	8285.566217	25.809549
188.350885	8290.411701	25.814567
188.315025	8303.230580	25.819584
188.563938	8305.696040	25.824602
188.923021	8301.313232	25.829620
188.652631	8316.082863	25.834637
189.073256	8323.120402	25.839655
189.320345	8328.350942	25.844672
189.152457	8341.733078	25.849690
189.494065	8342.896393	25.854708
189.671005	8359.600969	25.859725
189.719903	8358.514363	25.864743
190.156795	8366.767459	25.869760
190.322971	8393.625663	25.874778
190.300501	8392.313180	25.879796
190.394139	8398.551842	25.884813
190.932552	8409.373375	25.889831
190.791608	8431.183410	25.894848
190.721937	8433.661121	25.899866
191.168832	8441.541636	25.904884
191.378397	8467.922485	25.909901
191.518693	8461.343615	25.914919
191.536924	8466.088966	25.919936
191.742413	8494.952429	25.924954
191.877595	8497.353820	25.929972
191.683310	8522.405128	25.934989
192.223389	8535.636412	25.940007
192.555769	8549.563007	25.945024
192.548275	8574.813224	25.950042
192.736984	8573.693299	25.955060
192.752512	8601.004366	25.960077
193.141049	8612.349239	25.965095
193.565270	8629.969230	25.970112
193.798934	8634.619305	25.975130
194.359960	8639.523307	25.980148
194.573807	8653.269804	25.985165
194.971962	8656.207293	25.990183
195.326309	8657.796295	25.995200
195.324333	8656.214935	26.000218
195.708840	8644.125203	26.005236
195.561431	8643.704915	26.010253
196.045863	8650.149725	26.015271
195.858280	8671.194394	26.020288
196.006185	8674.027772	26.025306
196.240908	8674.618355	26.030324
196.038686	8682.132291	26.035341
196.518030	8696.287411	26.040359
196.574705	8706.819251	26.045376
196.639135	8719.146016	26.050394
197.029062	8734.560734	26.055412
197.311169	8738.476788	26.060429
197.401662	8739.638065	26.065447
197.857884	8758.049082	26.070464
197.658803	8773.114301	26.075482
198.163288	8765.195733	26.080500
198.252613	8789.062412	26.085517
198.145778	8803.512138	26.090535
198.627886	8809.797247	26.095552
198.935521	8820.603540	26.100570
198.944521	8827.021521	26.105588
199.035883	8836.719679	26.110605
199.443030	8856.840377	26.115623
199.385925	8863.669854	26.120640
199.112156	8877.370346	26.125658
199.542011	8893.872701	26.130676
199.542455	8914.485614	26.135693
199.913992	8934.379947	26.140711
200.407264	8948.390258	26.145728
200.382843	8969.732766	26.150746
200.505161	8973.167960	26.155764
200.667206	9003.843384	26.160781
200.962666	9014.632477	26.165799
201.270629	9033.571896	26.170816
201.431858	9043.318464	26.175834
201.736594	9051.138944	26.180852
201.649240	9080.401980	26.185869
201.744755	9080.115296	26.190887
202.412291	9096.099163	26.195904
202.199081	9115.320861	26.200922
202.623432	9135.252685	26.205940
202.550921	9155.570256	26.210957
202.941365	9168.997906	26.215975
203.293286	9176.758205	26.220992
203.088036	9196.230954	26.226010
203.656281	9216.119094	26.231028
203.815166	9222.034492	26.236045
204.299392	9231.301593	26.241063
204.978427	9236.041006	26.246080
204.736904	9245.200705	26.251098
204.956231	9246.975375	26.256116
205.341575	9264.446103	26.261133
205.157852	9272.234390	26.266151
205.505344	9285.482483	26.271168
205.359519	9304.813692	26.276186
205.592008	9303.888590	26.281204
206.121949	9325.179826	26.286221
206.239812	9335.373013	26.291239
206.508583	9344.746930	26.296256
206.650581	9363.939472	26.301274
206.980659	9370.327358	26.306292
207.169169	9386.780196	26.311309
207.193411	9400.893636	26.316327
207.475781	9408.139847	26.321344
207.525847	9423.767239	26.326362
208.149090	9434.246655	26.331380
208.341726	9441.987627	26.336397
208.430742	9467.567076	26.341415
208.639144	9467.430407	26.346432
208.633592	9484.814967	26.351450
209.105269	9503.270476	26.356468
208.975912	9512.422688	26.361485
209.154408	9526.811097	26.366503
209.801873	9549.865612	26.371520
209.382510	9553.830743	26.376538
209.860096	9563.337955	26.381556
210.272652	9583.938426	26.386573
210.309981	9601.623598	26.391591
210.888162	9595.421432	26.396608
210.751683	9612.899019	26.401626
211.315565	9623.439184	26.406644
211.641950	9630.514404	26.411661
211.465621	9646.791954	26.416679
211.950331	9647.978997	26.421696
211.756783	9670.640488	26.426714
211.959527	9668.000962	26.431732
212.367274	9689.738736	26.436749
212.280123	9695.285494	26.441767
212.711564	9705.757509	26.446784
212.596527	9723.996746	26.451802
212.757892	9736.022829	26.456820
212.720320	9750.196817	26.461837
213.132348	9777.767513	26.466855
213.757030	9789.803990	26.471872
213.933183	9804.058859	26.476890
214.001281	9803.453477	26.481908
214.439269	9813.866287	26.486925
214.345838	9826.462302	26.491943
215.115234	9840.931138	26.496960
215.322753	9856.928947	26.501978
215.371822	9854.365826	26.506996
215.545025	9865.703876	26.512013
215.485412	9866.470887	26.517031
215.844970	9893.501239	26.522048
215.783981	9901.279335	26.527066
216.132068	9918.596220	26.532084
216.398528	9937.662625	26.537101
216.779003	9945.321187	26.542119
217.676957	9953.466258	26.547136
217.614808	9961.768705	26.552154
217.907492	9952.190077	26.557172
218.005847	9952.546288	26.562189
218.073107	9982.772529	26.567207
218.468364	9976.662329	26.572224
218.362339	9988.629715	26.577242
218.721071	9994.756743	26.582260
218.790575	10004.339517	26.587277
218.685853	10020.491942	26.592295
219.259939	10036.562151	26.597312
219.241582	10058.568278	26.602330
219.430452	10057.261311	26.607348
219.532908	10078.500958	26.612365
219.760777	10098.161998	26.617383
219.998623	10100.244290	26.622400
219.636841	10120.373961	26.627418
219.826340	10153.832934	26.632436
220.435835	10167.989954	26.637453
220.639329	10190.099815	26.642471
220.723493	10208.264993	26.647488
220.912260	10236.677616	26.652506
221.099276	10257.889478	26.657524
222.158060	10269.962606	26.662541
221.807396	10302.797740	26.667559
222.403136	10295.934163	26.672576
222.203859	10326.021386	26.677594
222.461905	10338.149410	26.682612
223.056368	10340.615617	26.687629
223.091473	10364.141252	26.692647
223.489264	10377.617611	26.697664
223.802258	10393.944282	26.702682
223.775373	10401.773865	26.707700
224.145000	10416.049630	26.712717
224.264319	10422.830441	26.717735
225.018610	10441.799263	26.722752
224.750490	10462.874026	26.727770
225.174710	10462.178404	26.732788
225.538706	10455.430398	26.737805
225.454879	10481.794262	26.742823
225.638795	10499.091945	26.747840
225.988102	10494.894231	26.752858
226.267822	10513.609818	26.757876
226.350428	10523.055467	26.762893
226.051155	10538.364291	26.767911
226.571023	10552.877135	26.772928
226.562848	10571.772478	26.777946
226.802702	10606.551346	26.782964
227.236728	10607.021311	26.787981
227.228726	10639.204023	26.792999
227.664807	10641.489720	26.798016
227.438785	10667.747109	26.803034
227.937898	10677.996128	26.808052
228.636094	10690.843272	26.813069
228.652722	10705.415623	26.818087
229.162724	10728.735088	26.823104
229.471492	10726.850556	26.828122
229.263832	10757.307122	26.833140
229.786152	10750.880436	26.838157
229.911062	10777.528323	26.843175
229.974063	10793.280604	26.848192
230.607699	10807.886927	26.853210
230.908044	10817.538491	26.858228
231.437278	10831.438981	26.863245
231.719340	10828.147541	26.868263
231.785616	10825.389870	26.873280
231.936966	10844.006700	26.878298
232.077627	10860.342065	26.883316
232.434611	10860.552005	26.888333
232.388200	10857.316065	26.893351
232.862005	10877.608689	26.898368
233.096605	10885.877328	26.903386
233.068170	10884.967754	26.908404
233.139756	10908.655274	26.913421
233.164321	10908.739544	26.918439
233.639635	10923.054825	26.923456
233.838324	10946.318393	26.928474
233.613233	10967.455274	26.933492
234.036749	10978.957321	26.938509
234.552661	11008.135415	26.943527
234.613754	11015.695896	26.948544
234.717540	11034.940734	26.953562
234.886982	11058.176474	26.958580
235.439496	11076.246793	26.963597
235.538360	11086.937280	26.968615
235.652422	11099.236834	26.973632
235.891425	11121.782754	26.978650
236.366111	11146.918318	26.983668
236.922124	11148.610826	26.988685
236.997197	11155.931853	26.993703
237.268560	11182.418983	26.998720
237.579153	11186.422442	27.003738
237.338359	11191.924583	27.008756
237.725619	11207.873534	27.013773
237.546628	11217.047279	27.018791
237.996733	11236.323748	27.023808
238.125100	11247.892329	27.028826
238.452701	11272.937424	27.033844
238.860191	11279.181957	27.038861
238.932841	11311.117125	27.043879
239.312277	11320.451618	27.048896
239.809566	11332.301273	27.053914
239.954867	11355.171399	27.058932
240.153401	11345.425681	27.063949
240.158619	11377.290079	27.068967
240.468489	11389.789662	27.073984
241.018796	11397.690287	27.079002
241.048921	11426.308706	27.084020
241.455923	11424.682332	27.089037
241.381880	11448.526923	27.094055
241.354106	11460.162662	27.099072
241.682253	11481.930473	27.104090
241.852460	11512.646498	27.109108
241.915903	11528.970494	27.114125
242.619053	11559.063310	27.119143
242.743774	11572.468764	27.124160
242.836759	11592.074543	27.129178
242.871713	11619.536344	27.134196
243.160344	11633.431260	27.139213
243.693619	11663.459666	27.144231
243.938192	11676.357923	27.149248
244.321927	11697.679371	27.154266
244.394743	11709.658963	27.159284
245.074859	11721.702135	27.164301
245.125383	11742.821153	27.169319
245.554187	11762.382677	27.174336
246.212689	11775.155027	27.179354
245.897972	11796.549571	27.184372
246.179936	11799.613454	27.189389
246.604181	11810.074117	27.194407
246.765445	11832.175797	27.199424
247.022363	11839.928617	27.204442
247.198978	11859.715823	27.209460
247.362149	11871.536711	27.214477
247.845098	11891.610825	27.219495
247.788191	11911.662199	27.224512
248.193783	11913.436035	27.229530
248.257204	11945.813995	27.234548
248.777292	11947.810633	27.239565
248.848658	11963.222774	27.244583
248.936888	11978.954952	27.249600
249.410602	11990.856306	27.254618
249.477129	12008.672659	27.259636
249.623967	12027.999854	27.264653
250.064695	12051.694472	27.269671
250.270794	12073.626822	27.274688
250.853604	12079.158183	27.279706
250.291525	12097.124812	27.284724
250.635290	12098.959688	27.289741
251.139623	12123.610446	27.294759
251.374180	12144.314813	27.299776
251.668161	12162.451453	27.304794
251.828586	12188.298629	27.309812
252.399808	12194.151050	27.314829
252.307287	12211.490818	27.319847
252.616249	12232.802702	27.324864
253.170515	12250.800361	27.329882
252.907705	12264.977182	27.334900
253.444955	12275.494342	27.339917
253.645495	12294.771798	27.344935
253.605982	12310.640975	27.349952
254.154967	12330.485739	27.354970
254.353430	12352.912049	27.359988
254.575804	12379.764265	27.365005
254.688729	12398.741562	27.370023
255.062524	12412.997106	27.375040
255.460796	12427.128728	27.380058
255.460116	12449.452717	27.385076
255.692740	12471.866673	27.390093
256.004800	12487.265973	27.395111
256.322359	12510.351047	27.400128
256.726501	12522.986094	27.405146
256.993826	12543.337875	27.410164
257.376909	12560.779338	27.415181
257.546320	12581.647387	27.420199
257.608675	12600.865394	27.425216
258.246481	12608.128917	27.430234
258.447127	12638.345888	27.435252
258.858809	12644.495081	27.440269
259.126517	12651.952605	27.445287
259.331002	12667.730724	27.450304
259.860742	12679.812013	27.455322
259.674428	12700.036179	27.460340
260.064646	12706.680383	27.465357
260.175909	12715.861701	27.470375
260.418901	12743.525365	27.475392
260.762372	12755.702524	27.480410
261.088340	12770.992845	27.485428
261.329470	12796.550923	27.490445
261.871044	12799.339068	27.495463
261.800115	12828.307223	27.500480
261.881205	12836.391626	27.505498
261.940007	12862.228594	27.510516
262.112348	12879.898634	27.515533
262.939021	12900.422679	27.520551
262.943765	12915.763360	27.525568
263.313679	12927.312041	27.530586
263.157721	12959.442176	27.535604
263.648944	12981.855714	27.540621
263.780420	12992.451529	27.545639
263.862181	13014.304988	27.550656
264.331060	13032.383011	27.555674
264.466082	13058.553230	27.560692
265.047217	13063.023458	27.565709
265.906182	13056.825241	27.570727
265.756751	13085.221641	27.575744
266.304884	13090.419840	27.580762
266.654504	13106.859121	27.585780
266.687748	13103.658906	27.590797
266.719005	13118.255544	27.595815
267.288021	13132.478684	27.600832
267.329525	13130.317470	27.605850
267.458631	13161.758410	27.610868
267.767139	13166.567796	27.615885
268.018473	13192.702587	27.620903
268.049168	13209.382514	27.625920
268.409267	13221.040135	27.630938
268.589498	13252.643730	27.635956
269.235210	13272.652113	27.640973
269.352622	13277.459423	27.645991
269.528561	13303.247081	27.651008
269.695118	13308.751866	27.656026
270.190850	13331.764356	27.661044
270.484609	13352.768813	27.666061
270.666915	13363.984452	27.671079
270.856950	13383.204251	27.676096
271.027079	13401.779801	27.681114
271.397150	13427.912700	27.686132
271.296583	13446.335837	27.691149
271.870866	13460.001227	27.696167
271.674731	13483.992638	27.701184
272.312552	13506.124606	27.706202
272.512205	13540.345118	27.711220
272.900728	13560.704822	27.716237
273.785313	13578.607332	27.721255
273.417262	13601.856272	27.726272
274.021909	13608.960751	27.731290
274.233143	13615.782757	27.736308
274.026296	13651.069990	27.741325
274.980552	13655.835160	27.746343
275.318199	13680.593142	27.751360
275.471050	13687.159992	27.756378
275.450227	13703.043185	27.761396
275.905428	13718.498948	27.766413
276.173675	13739.981398	27.771431
276.020665	13752.838222	27.776448
276.746636	13783.142688	27.781466
276.560377	13800.785636	27.786484
276.941160	13816.873076	27.791501
277.530964	13846.490898	27.796519
277.433959	13870.600544	27.801536
277.576047	13897.176970	27.806554
277.918222	13907.691921	27.811572
278.031365	13931.301462	27.816589
278.426796	13958.471407	27.821607
278.682066	13989.766122	27.826624
278.798430	14006.032187	27.831642
279.237232	14026.637289	27.836660
279.597616	14049.001125	27.841677
280.060384	14076.427016	27.846695
280.163248	14100.828021	27.851712
280.603379	14115.729841	27.856730
281.118327	14138.034341	27.861748
281.247923	14155.203717	27.866765
281.798338	14157.043703	27.871783
281.856754	14183.484097	27.876800
282.155272	14198.551840	27.881818
282.459106	14205.566684	27.886836
283.022631	14222.053570	27.891853
283.551572	14225.636327	27.896871
283.895217	14236.412330	27.901888
284.122453	14243.659523	27.906906
284.235467	14256.382365	27.911924
284.560607	14269.322137	27.916941
284.997045	14271.359591	27.921959
284.883246	14299.959306	27.926976
285.048177	14304.260470	27.931994
285.433217	14327.492723	27.937012
285.267035	14341.806912	27.942029
285.461335	14368.152758	27.947047
285.541898	14394.311409	27.952064
285.862567	14414.031447	27.957082
286.243686	14437.046037	27.962100
286.659967	14463.471800	27.967117
287.186558	14494.049065	27.972135
287.185573	14525.468079	27.977152
287.484223	14546.516992	27.982170
287.479536	14562.594916	27.987188
288.068181	14594.044579	27.992205
288.227325	14613.282165	27.997223
288.637410	14640.479721	28.002240
288.909341	14665.047846	28.007258
289.332632	14693.188760	28.012276
289.294077	14721.149348	28.017293
290.150539	14733.773783	28.022311
290.427642	14751.742415	28.027328
290.557324	14773.725860	28.032346
291.310348	14790.278416	28.037364
291.026967	14810.865055	28.042381
291.509672	14827.863702	28.047399
291.599286	14850.173852	28.052416
292.233753	14854.124905	28.057434
292.455088	14883.889961	28.062452
292.657304	14895.794949	28.067469
293.536614	14920.664244	28.072487
293.673907	14927.423932	28.077504
293.772043	14945.450048	28.082522
294.402941	14969.611719	28.087540
294.358929	14993.515508	28.092557
294.577496	14989.278572	28.097575
295.107474	15012.311242	28.102592
294.922545	15037.759706	28.107610
295.451956	15035.774158	28.112628
295.235009	15069.065654	28.117645
295.851661	15091.410052	28.122663
295.754616	15116.793764	28.127680
296.031269	15128.069466	28.132698
296.526355	15155.915687	28.137716
296.194800	15192.787663	28.142733
296.635300	15213.377562	28.147751
297.466676	15236.972663	28.152768
298.054687	15243.573373	28.157786
298.845797	15250.549815	28.162804
298.621691	15270.033226	28.167821
299.044243	15274.696589	28.172839
299.254067	15296.042233	28.177856
299.306990	15313.566035	28.182874
299.486440	15330.404847	28.187892
299.801026	15364.324748	28.192909
300.184385	15380.312949	28.197927
300.358742	15398.707700	28.202944
300.498955	15428.167108	28.207962
300.716989	15451.864716	28.212980
300.966008	15487.772967	28.217997
301.283968	15515.354710	28.223015
301.810414	15547.479327	28.228032
301.973023	15572.585340	28.233050
302.519602	15601.323924	28.238068
303.074197	15626.545678	28.243085
303.256141	15626.057340	28.248103
303.734062	15652.840334	28.253120
304.308197	15659.557495	28.258138
305.055585	15681.074363	28.263156
304.926283	15703.561562	28.268173
304.960502	15717.385611	28.273191
305.376157	15725.135390	28.278208
305.439435	15761.484057	28.283226
305.931580	15776.588137	28.288244
306.020327	15805.158761	28.293261
306.390111	15814.628844	28.298279
306.811473	15829.761577	28.303296
306.653785	15855.816806	28.308314
307.221791	15876.768721	28.313332
307.255332	15911.341029	28.318349
307.554015	15936.110046	28.323367
307.816363	15956.773818	28.328384
307.936358	15981.139551	28.333402
308.543645	16006.673766	28.338420
308.574467	16044.133051	28.343437
309.077123	16069.213041	28.348455
309.370545	16106.889848	28.353472
309.526008	16120.654587	28.358490
310.144118	16143.359692	28.363508
310.198445	16177.252788	28.368525
310.888822	16200.160412	28.373543
311.236648	16213.341295	28.378560
311.310404	16256.004877	28.383578
311.719649	16261.172380	28.388596
311.822300	16290.869515	28.393613
312.480397	16301.073001	28.398631
312.707063	16312.958460	28.403648
312.778054	16349.953079	28.408666
313.372332	16360.721836	28.413684
313.479776	16389.322841	28.418701
313.614296	16411.408433	28.423719
314.398892	16425.935301	28.428736
314.520138	16447.182790	28.433754
314.932196	16466.591816	28.438772
315.116130	16492.694847	28.443789
315.229686	16518.199549	28.448807
315.700581	16538.441138	28.453824
316.184851	16556.909723	28.458842
316.865545	16579.747220	28.463860
317.019654	16589.415130	28.468877
317.549597	16596.620218	28.473895
318.168597	16609.407274	28.478912
318.433704	16618.528623	28.483930
318.674385	16641.242451	28.488948
318.830149	16653.336502	28.493965
319.154263	16672.896603	28.498983
319.540025	16676.704129	28.504000
319.713430	16710.142841	28.509018
320.265120	16718.926084	28.514036
320.279206	16728.750637	28.519053
320.601377	16752.492109	28.524071
321.014134	16768.407195	28.529088
320.978734	16787.881437	28.534106
321.369849	16809.472412	28.539124
321.495125	16835.717250	28.544141
321.500372	16857.701255	28.549159
322.200020	16881.444775	28.554176
322.110432	16913.995587	28.559194
322.356913	16940.258489	28.564212
322.920636	16970.272009	28.569229
322.999174	16997.076106	28.574247
323.527475	17014.201892	28.579264
323.670641	17041.695330	28.584282
324.447240	17073.362229	28.589300
324.472310	17107.838173	28.594317
324.885228	17131.540768	28.599335
325.202612	17158.855675	28.604352
325.497881	17187.629985	28.609370
326.288194	17208.396328	28.614388
326.315162	17227.054530	28.619405
326.931118	17253.762998	28.624423
327.392139	17274.239400	28.629440
327.600522	17289.830719	28.634458
327.823280	17311.375015	28.639476
328.546618	17330.712494	28.644493
328.607244	17350.146944	28.649511
329.366452	17349.656721	28.654528
329.025009	17376.738038	28.659546
329.418675	17394.500638	28.664564
329.710049	17409.469426	28.669581
329.440422	17434.981978	28.674599
329.953072	17467.233460	28.679616
330.271720	17493.268484	28.684634
330.607484	17510.014885	28.689652
330.813484	17540.934721	28.694669
330.896714	17571.114753	28.699687
331.332436	17592.348345	28.704704
331.387698	17647.031593	28.709722
331.483874	17668.076881	28.714740
332.130796	17700.913346	28.719757
332.562671	17740.308454	28.724775
332.955308	17775.056434	28.729792
333.140343	17808.162396	28.734810
333.546094	17834.754972	28.739828
333.657624	17876.917196	28.744845
334.378620	17914.030074	28.749863
335.547979	17933.175975	28.754880
336.041644	17959.713418	28.759898
336.289358	17975.521205	28.764916
336.503864	17996.033909	28.769933
336.793439	18010.671676	28.774951
337.122526	18032.628770	28.779968
337.313199	18052.270934	28.784986
337.637504	18075.312714	28.790004
338.027287	18094.069260	28.795021
337.868599	18127.752727	28.800039
338.628648	18147.027505	28.805056
338.627881	18167.648363	28.810074
338.971494	18195.342023	28.815092
339.748325	18217.554413	28.820109
339.964362	18243.153102	28.825127
340.264814	18273.990446	28.830144
340.469692	18301.088674	28.835162
340.683279	18326.085909	28.840180
341.161764	18370.107572	28.845197
341.351180	18389.815325	28.850215
342.065994	18407.390112	28.855232
342.208514	18442.676699	28.860250
342.227082	18477.768150	28.865268
342.919383	18494.326513	28.870285
342.930101	18528.366932	28.875303
343.943923	18545.357597	28.880320
343.957590	18575.547118	28.885338
344.624979	18605.825055	28.890356
344.987481	18617.867813	28.895373
344.927946	18656.029321	28.900391
345.470598	18670.041923	28.905408
345.735118	18693.701260	28.910426
345.935149	18730.623109	28.915444
346.667769	18748.380495	28.920461
346.346107	18778.096257	28.925479
347.131905	18802.199885	28.930496
347.513591	18816.626873	28.935514
347.666375	18840.071547	28.940532
348.025398	18857.398800	28.945549
348.450654	18881.635598	28.950567
348.946661	18908.400286	28.955584
348.945386	18932.257859	28.960602
349.392507	18950.493674	28.965620
350.003792	18973.970220	28.970637
350.011439	19001.571596	28.975655
350.341870	19027.093892	28.980672
350.506081	19050.491783	28.985690
350.805859	19079.925222	28.990708
351.184647	19107.388112	28.995725
351.004377	19154.024620	29.000743
352.002859	19178.326850	29.005760
352.235296	19221.645974	29.010778
352.331522	19248.805291	29.015796
352.892492	19279.496804	29.020813
352.905801	19321.327766	29.025831
353.166267	19349.922631	29.030848
353.615505	19385.315636	29.035866
354.118647	19424.109894	29.040884
354.392890	19463.273432	29.045901
354.548341	19507.350566	29.050919
354.843115	19543.148500	29.055936
355.258800	19582.537066	29.060954
355.548716	19613.369287	29.065972
356.614926	19641.759121	29.070989
357.087261	19691.493578	29.076007
357.050098	19724.726030	29.081024
357.765879	19756.382505	29.086042
357.989844	19786.662520	29.091060
358.473720	19816.453882	29.096077
358.998100	19850.842545	29.101095
359.604246	19859.983321	29.106112
359.970743	19891.314578	29.111130
360.106830	19922.205388	29.116148
360.988004	19928.928466	29.121165
361.052382	19963.666299	29.126183
361.694898	19985.530922	29.131200
361.977762	20012.891382	29.136218
362.023337	20024.332888	29.141236
362.371391	20050.946317	29.146253
362.375629	20086.181864	29.151271
363.197241	20099.944193	29.156288
363.574438	20132.342876	29.161306
363.807419	20152.062449	29.166324
364.701413	20165.291971	29.171341
364.877895	20197.253414	29.176359
365.329002	20194.121691	29.181376
365.986772	20218.182945	29.186394
366.088910	20248.118645	29.191412
366.277767	20276.129675	29.196429
366.527496	20291.442568	29.201447
366.995788	20306.671036	29.206464
367.367859	20315.411520	29.211482
367.275523	20351.473013	29.216500
367.913954	20356.145274	29.221517
368.086037	20381.833616	29.226535
368.548519	20413.888533	29.231552
368.890563	20431.138337	29.236570
369.030001	20455.118348	29.241588
369.527498	20467.418237	29.246605
369.200359	20502.884713	29.251623
369.971764	20543.462130	29.256640
370.332677	20577.752826	29.261658
370.337035	20602.943759	29.266676
370.624298	20638.466999	29.271693
370.934107	20673.738653	29.276711
371.334852	20721.667395	29.281728
371.311330	20750.876306	29.286746
371.904629	20796.216663	29.291764
372.428543	20829.547910	29.296781
372.444786	20871.874356	29.301799
373.242836	20909.721989	29.306816
373.756917	20947.477926	29.311834
373.978999	20997.919911	29.316852
374.353787	21025.386804	29.321869
374.744950	21067.504401	29.326887
375.343072	21093.232343	29.331904
375.916924	21124.908689	29.336922
376.185790	21171.677688	29.341940
376.688908	21197.084649	29.346957
376.866828	21235.528040	29.351975
377.259945	21264.214729	29.356992
377.981894	21297.181487	29.362010
378.004585	21335.291512	29.367028
378.511291	21368.221044	29.372045
378.616091	21407.088404	29.377063
378.752647	21438.535781	29.382080
379.188365	21483.456671	29.387098
379.484165	21537.522518	29.392116
380.233943	21561.022625	29.397133
380.461530	21610.543435	29.402151
381.134862	21640.125748	29.407168
381.449878	21674.949103	29.412186
381.823464	21711.671530	29.417204
382.309529	21746.918291	29.422221
382.209176	21798.815334	29.427239
382.846278	21825.963019	29.432256
383.043088	21861.080489	29.437274
384.063256	21896.070000	29.442292
384.513873	21929.545209	29.447309
384.847250	21967.392240	29.452327
385.157232	21996.293559	29.457344
385.972449	22023.667602	29.462362
386.237405	22051.116765	29.467380
386.586466	22083.089190	29.472397
386.684769	22108.998456	29.477415
386.972955	22140.716849	29.482432
387.328488	22162.270691	29.487450
387.681083	22198.143036	29.492468
388.038488	22221.795649	29.497485
388.321981	22253.229899	29.502503
388.528424	22280.548588	29.507520
389.042511	22306.676260	29.512538
389.527175	22341.622914	29.517556
390.024838	22375.992611	29.522573
390.387540	22408.280145	29.527591
391.020803	22441.305960	29.532608
391.290110	22467.112166	29.537626
391.323125	22506.236253	29.542644
392.052879	22533.049830	29.547661
392.486199	22557.628918	29.552679
392.837444	22588.786820	29.557696
393.649071	22610.574995	29.562714
393.932245	22638.195553	29.567732
394.451317	22655.570817	29.572749
395.781455	22662.574456	29.577767
396.903650	22662.763523	29.582784
397.263185	22672.129553	29.587802
397.468126	22683.245933	29.592820
398.024846	22675.666845	29.597837
398.269484	22676.589609	29.602855
398.035954	22678.038298	29.607872
398.332855	22697.208586	29.612890
398.495706	22719.684709	29.617908
399.072356	22733.714449	29.622925
399.337477	22760.956094	29.627943
399.704694	22779.659236	29.632960
400.216406	22786.635802	29.637978
400.251823	22822.126895	29.642996
400.881389	22829.995219	29.648013
400.894388	22858.135733	29.653031
400.822098	22884.147486	29.658048
401.480082	22898.914255	29.663066
401.584030	22932.941468	29.668084
401.877196	22964.566201	29.673101
402.163106	23004.102548	29.678119
402.821775	23039.426301	29.683136
403.668659	23059.693248	29.688154
404.045281	23092.533683	29.693172
404.234588	23119.955008	29.698189
404.577299	23144.358044	29.703207
404.570688	23181.861230	29.708224
405.002756	23207.168540	29.713242
405.588491	23235.846240	29.718260
405.829386	23287.480326	29.723277
406.290638	23318.529194	29.728295
406.451016	23358.952860	29.733312
407.154102	23396.083549	29.738330
407.488842	23426.410009	29.743348
407.871316	23459.652772	29.748365
408.168916	23487.048812	29.753383
408.724215	23524.861846	29.758400
408.795835	23546.208389	29.763418
409.216702	23592.209664	29.768436
409.724548	23621.752743	29.773453
410.257911	23653.958912	29.778471
410.125019	23698.396158	29.783488
410.877355	23733.094501	29.788506
410.685163	23768.085974	29.793524
411.140078	23818.014629	29.798541
411.721278	23853.608538	29.803559
412.185046	23903.697529	29.808576
412.729260	23940.448351	29.813594
413.375710	23988.202120	29.818612
413.374898	24028.637411	29.823629
413.640216	24062.412106	29.828647
413.946062	24111.874691	29.833664
415.121855	24142.726257	29.838682
415.250901	24187.468935	29.843700
415.588152	24221.424708	29.848717
416.535562	24262.817835	29.853735
416.970906	24303.577404	29.858752
417.417353	24338.001263	29.863770
417.944379	24378.008323	29.868788
418.295481	24397.773849	29.873805
418.742743	24429.736933	29.878823
418.945655	24470.502451	29.883840
419.697985	24498.506016	29.888858
419.979225	24542.717359	29.893876
420.251524	24582.589852	29.898893
420.858383	24614.526305	29.903911
421.115886	24646.598042	29.908928
421.630934	24677.638628	29.913946
422.421197	24701.236218	29.918964
422.491239	24737.939173	29.923981
423.232211	24777.632717	29.928999
423.371265	24814.628133	29.934016
423.939748	24844.904300	29.939034
424.214363	24886.832406	29.944052
424.527606	24915.877162	29.949069
424.676186	24953.246348	29.954087
425.994017	24974.432497	29.959104
426.521175	24996.407138	29.964122
427.107017	25025.693044	29.969140
427.574163	25043.612509	29.974157
428.185063	25067.629945	29.979175
428.029280	25092.449393	29.984192
428.584140	25121.192131	29.989210
428.749762	25156.803167	29.994228
429.178236	25188.915713	29.999245
429.531434	25212.956305	30.004263
429.604343	25247.791401	30.009280
430.077388	25281.460742	30.014298
430.636939	25322.231483	30.019316
430.693348	25348.760851	30.024333
431.057741	25386.685918	30.029351
431.267235	25427.998750	30.034368
431.819401	25465.779863	30.039386
432.026204	25503.152084	30.044404
432.354579	25543.226798	30.049421
432.991574	25575.237575	30.054439
433.332404	25627.285553	30.059456
433.449980	25668.468696	30.064474
434.110654	25708.405802	30.069492
434.598847	25752.459894	30.074509
434.919447	25798.773404	30.079527
435.100485	25832.013021	30.084544
435.644504	25882.781594	30.089562
436.098026	25926.944889	30.094580
436.825242	25988.219819	30.099597
437.423181	26014.671105	30.104615
437.723520	26064.552620	30.109632
438.071691	26111.667774	30.114650
438.631739	26157.910297	30.119668
438.806951	26201.219794	30.124685
439.166155	26242.109874	30.129703
439.798396	26303.584697	30.134720
440.272521	26341.228255	30.139738
441.015878	26383.020207	30.144756
441.484803	26428.550867	30.149773
442.227580	26465.064724	30.154791
442.245612	26512.736277	30.159808
442.974536	26538.784678	30.164826
443.568966	26576.764932	30.169844
443.719126	26614.863321	30.174861
444.860073	26647.108724	30.179879
445.472217	26674.920209	30.184896
446.160429	26705.309238	30.189914
446.755135	26729.940745	30.194932
447.002385	26753.571941	30.199949
447.497929	26776.694852	30.204967
447.861126	26815.275024	30.209984
448.291537	26821.729023	30.215002
448.489235	26847.649049	30.220020
449.090521	26882.684770	30.225037
449.334089	26903.881549	30.230055
449.320611	26938.842790	30.235072
449.953968	26974.645692	30.240090
450.564060	27022.260673	30.245108
450.647216	27066.269438	30.250125
451.243755	27091.240772	30.255143
451.815284	27126.346368	30.260160
452.113950	27159.076788	30.265178
452.793191	27197.561044	30.270196
452.775176	27236.928571	30.275213
453.240964	27273.091307	30.280231
453.744929	27317.424499	30.285248
454.283376	27358.870304	30.290266
454.802597	27398.603300	30.295284
455.008369	27441.919139	30.300301
455.872909	27474.827930	30.305319
456.189236	27502.408276	30.310336
456.369530	27542.994523	30.315354
456.914160	27572.621764	30.320372
457.546555	27596.366960	30.325389
458.230225	27625.100755	30.330407
458.120737	27660.547637	30.335424
458.879031	27694.058410	30.340442
459.467818	27724.663749	30.345460
459.776566	27763.123283	30.350477
460.225997	27795.728550	30.355495
460.820899	27845.458344	30.360512
460.960524	27880.426380	30.365530
461.592886	27911.039313	30.370548
461.864949	27952.648836	30.375565
462.376532	27995.364337	30.380583
462.680521	28044.130998	30.385600
463.036949	28073.910475	30.390618
463.354659	28115.464294	30.395636
463.750528	28168.162512	30.400653
464.544934	28208.707753	30.405671
465.061314	28256.513064	30.410688
465.052484	28294.922021	30.415706
465.699123	28346.506159	30.420724
465.926098	28393.511755	30.425741
466.493687	28434.074781	30.430759
467.307691	28489.375328	30.435776
467.407548	28540.804505	30.440794
468.237546	28583.604780	30.445812
468.507459	28630.345782	30.450829
469.339779	28658.532975	30.455847
470.127288	28709.582098	30.460864
470.323233	28747.467834	30.465882
471.100529	28786.234940	30.470900
471.438409	28828.728167	30.475917
471.764064	28868.768231	30.480935
472.190806	28909.901714	30.485952
472.294985	28956.640112	30.490970
473.148628	28988.962767	30.495988
473.143495	29040.900350	30.501005
473.644436	29086.237982	30.506023
474.256410	29129.944326	30.511040
474.840866	29186.349124	30.516058
475.308282	29228.193972	30.521076
475.639237	29278.729793	30.526093
477.515678	29284.876436	30.531111
478.331368	29316.753503	30.536128
478.751992	29338.190019	30.541146
479.706042	29351.111962	30.546164
480.085949	29384.883502	30.551181
480.471428	29405.895478	30.556199
480.856553	29423.125298	30.561216
481.037421	29456.731700	30.566234
481.271232	29476.764056	30.571252
481.275313	29501.168442	30.576269
481.620441	29529.638055	30.581287
481.891485	29560.519684	30.586304
481.838934	29605.937475	30.591322
482.717891	29633.323082	30.596340
482.747541	29681.928752	30.601357
483.265491	29720.682666	30.606375
483.764613	29750.943644	30.611392
483.914405	29804.490103	30.616410
484.230665	29840.302573	30.621428
484.695937	29887.299737	30.626445
485.438516	29922.648910	30.631463
486.228019	29977.000224	30.636480
486.726242	30016.046388	30.641498
487.444010	30048.276174	30.646516
487.922414	30105.016243	30.651533
488.102096	30146.608266	30.656551
488.621294	30181.036948	30.661568
489.268156	30232.471007	30.666586
489.751412	30276.933778	30.671604
490.313755	30323.757558	30.676621
490.670054	30358.173161	30.681639
490.909113	30407.308692	30.686656
491.311645	30463.010878	30.691674
491.869048	30508.073968	30.696692
492.312789	30559.966941	30.701709
492.759302	30612.601955	30.706727
493.413244	30665.684794	30.711744
493.875877	30724.139539	30.716762
494.187485	30768.891036	30.721780
494.562658	30821.629497	30.726797
495.263583	30869.573837	30.731815
495.592314	30931.587356	30.736832
496.051462	30983.610030	30.741850
496.682823	31041.928705	30.746868
497.201938	31104.309725	30.751885
497.632456	31155.902503	30.756903
498.338631	31211.965500	30.761920
498.469695	31269.233028	30.766938
498.824998	31316.921658	30.771956
499.336184	31386.392803	30.776973
500.015848	31438.203690	30.781991
500.699498	31492.621028	30.787008
501.346414	31565.053350	30.792026
502.053831	31610.626733	30.797044
502.779183	31670.381144	30.802061
502.886600	31726.457731	30.807079
503.724068	31763.234798	30.812096
504.234369	31808.775504	30.817114
504.606016	31869.989763	30.822132
505.050186	31916.368789	30.827149
505.847552	31968.257169	30.832167
506.192722	32012.198126	30.837184
506.776543	32058.071419	30.842202
507.195009	32108.228469	30.847220
507.590119	32158.595873	30.852237
508.020640	32209.624523	30.857255
508.348318	32253.538960	30.862272
508.578800	32310.789542	30.867290
509.176323	32351.351218	30.872308
510.082698	32391.797600	30.877325
510.663460	32435.544537	30.882343
511.399489	32487.839956	30.887360
511.843384	32534.056835	30.892378
512.312294	32573.235121	30.897396
512.813751	32620.503880	30.902413
513.154717	32665.290533	30.907431
513.318304	32704.788876	30.912448
513.906450	32760.825506	30.917466
514.520544	32805.944185	30.922484
515.342339	32857.327072	30.927501
515.659346	32893.368330	30.932519
516.720709	32936.073795	30.937536
517.072746	32977.681772	30.942554
517.596541	33025.700014	30.947572
518.496071	33058.092767	30.952589
519.042462	33104.595987	30.957607
519.810861	33144.339525	30.962624
519.914439	33192.064211	30.967642
520.200815	33228.240333	30.972660
520.757777	33269.851084	30.977677
521.032373	33309.681551	30.982695
521.874626	33350.501472	30.987712
521.959999	33402.974355	30.992730
522.483687	33449.333985	30.997748
522.905583	33501.783530	31.002765
523.257324	33564.238340	31.007783
523.964798	33611.765586	31.012800
524.262110	33663.485151	31.017818
524.795918	33719.834762	31.022836
525.553121	33779.683161	31.027853
526.086469	33830.564866	31.032871
526.676645	33881.768711	31.037888
527.095059	33928.404970	31.042906
527.940053	33979.950013	31.047924
528.623272	34024.761494	31.052941
528.812034	34084.792958	31.057959
529.473022	34140.455357	31.062976
529.719274	34188.694574	31.067994
529.960824	34230.477775	31.073012
530.375394	34300.239804	31.078029
530.557380	34367.457017	31.083047
531.823286	34417.735159	31.088064
532.271958	34488.928656	31.093082
532.365299	34540.454852	31.098100
533.298914	34600.996959	31.103117
533.618997	34661.463595	31.108135
534.267944	34708.246611	31.113152
534.670775	34787.795924	31.118170
535.337410	34829.394690	31.123188
536.022057	34887.538725	31.128205
536.347494	34954.103295	31.133223
536.899208	35005.010888	31.138240
537.165692	35061.511663	31.143258
537.678541	35116.368539	31.148276
538.374931	35171.555801	31.153293
538.667313	35225.245293	31.158311
539.366793	35291.193556	31.163328
539.551115	35354.277651	31.168346
540.528505	35410.311670	31.173364
541.337401	35462.980065	31.178381
541.524521	35521.831421	31.183399
542.435959	35562.369869	31.188416
542.984355	35623.904034	31.193434
543.578116	35680.293290	31.198452
544.490108	35725.572670	31.203469
544.550628	35785.482474	31.208487
545.284135	35828.941280	31.213504
545.571482	35895.843582	31.218522
546.257562	35948.815271	31.223540
547.042887	35997.125202	31.228557
547.261230	36056.838994	31.233575
548.046770	36090.632162	31.238592
548.668287	36153.778916	31.243610
549.271328	36204.795499	31.248628
549.987028	36256.137990	31.253645
550.297899	36314.579849	31.258663
550.804696	36358.935378	31.263680
551.600479	36426.017380	31.268698
552.037660	36467.194823	31.273716
552.838058	36516.183366	31.278733
552.650402	36582.298494	31.283751
553.584929	36638.605171	31.288768
554.169219	36691.519739	31.293786
554.395757	36753.656395	31.298804
554.884594	36808.577816	31.303821
555.423646	36860.893118	31.308839
556.213135	36927.678563	31.313856
556.923648	36991.263634	31.318874
557.150836	37034.519250	31.323892
557.814384	37114.320296	31.328909
558.185053	37178.512029	31.333927
558.586658	37226.087237	31.338944
559.229011	37292.323652	31.343962
559.704309	37356.675988	31.348980
560.736006	37415.257562	31.353997
561.094878	37484.988104	31.359015
561.675825	37547.345587	31.364032
562.391509	37605.613932	31.369050
562.889131	37670.121579	31.374068
563.504297	37732.510560	31.379085
563.643404	37803.655469	31.384103
564.468182	37864.598808	31.389120
565.076253	37919.227352	31.394138
565.658821	37982.861765	31.399156
566.322447	38028.038695	31.404173
566.908865	38078.439210	31.409191
567.334173	38135.837958	31.414208
567.893157	38191.999926	31.419226
568.342053	38255.653500	31.424244
569.192476	38311.750532	31.429261
569.336371	38365.773273	31.434279
570.035403	38420.936094	31.439296
570.835740	38473.899108	31.444314
570.868636	38536.792172	31.449332
571.245677	38593.244617	31.454349
571.769489	38655.795039	31.459367
572.440600	38723.025866	31.464384
572.993305	38797.380965	31.469402
573.522947	38866.547573	31.474420
573.943599	38924.244596	31.479437
574.380116	39002.367224	31.484455
575.272053	39072.200742	31.489472
575.905480	39138.512031	31.494490
576.166729	39217.904543	31.499508
576.836373	39282.455581	31.504525
577.533496	39352.926792	31.509543
578.451975	39422.101543	31.514560
579.186795	39486.108413	31.519578
579.482914	39544.174286	31.524596
580.367573	39599.771828	31.529613
580.821176	39673.039557	31.534631
581.624255	39733.688728	31.539648
582.566384	39791.778721	31.544666
583.337146	39842.741730	31.549684
584.043265	39892.846302	31.554701
584.536883	39952.441689	31.559719
585.023484	40004.145857	31.564736
585.653798	40054.870096	31.569754
586.189341	40127.532224	31.574772
587.042139	40175.893826	31.579789
587.143781	40233.452121	31.584807
587.828787	40284.083176	31.589824
588.658915	40342.724318	31.594842
588.801583	40404.824618	31.599860
589.410894	40461.463888	31.604877
590.166940	40523.053772	31.609895
590.804279	40581.086179	31.614912
591.229392	40636.440157	31.619930
591.613358	40712.762295	31.624948
592.509351	40769.845803	31.629965
592.718844	40837.548003	31.634983
593.360135	40901.964600	31.640000
594.117808	40961.127200	31.645018
594.723921	41030.681506	31.650036
595.329876	41087.509472	31.655053
595.995882	41148.469362	31.660071
596.382425	41204.853238	31.665088
597.069740	41274.916027	31.670106
597.553067	41334.744962	31.675124
598.370945	41391.048147	31.680141
599.407121	41453.830031	31.685159
600.103984	41505.128333	31.690176
600.480328	41556.603995	31.695194
601.190653	41610.985228	31.700212
601.732289	41667.109363	31.705229
601.793645	41727.054171	31.710247
602.464746	41787.760033	31.715264
603.108544	41829.308690	31.720282
603.299856	41898.030461	31.725300
603.951178	41946.097958	31.730317
604.584278	42021.162400	31.735335
604.951408	42089.708689	31.740352
606.177283	42143.719322	31.745370
606.206415	42209.875363	31.750388
606.612090	42278.088219	31.755405
607.478525	42349.855412	31.760423
608.254345	42421.186267	31.765440
608.781642	42476.848487	31.770458
609.444377	42558.935217	31.775476
610.089675	42614.944995	31.780493
610.522893	42677.272197	31.785511
610.730425	42750.470806	31.790528
611.532488	42804.308113	31.795546
612.140730	42898.565258	31.800564
612.579862	42963.681035	31.805581
613.490784	43042.232305	31.810599
614.049766	43112.310386	31.815616
614.989856	43183.129294	31.820634
614.966018	43266.543170	31.825652
615.523873	43337.104973	31.830669
616.277220	43419.708156	31.835687
616.712417	43498.838813	31.840704
617.286973	43578.083285	31.845722
617.917866	43660.306490	31.850740
618.441814	43743.345214	31.855757
619.116896	43823.486463	31.860775
619.755696	43907.952475	31.865792
620.631146	43988.441130	31.870810
621.077900	44068.619868	31.875828
621.782702	44143.906080	31.880845
622.555512	44235.380839	31.885863
623.074010	44311.883587	31.890880
623.925966	44380.440607	31.895898
624.581114	44463.032843	31.900916
625.301102	44535.110024	31.905933
625.974792	44602.592164	31.910951
626.566314	44672.261247	31.915968
627.254672	44757.067354	31.920986
627.620545	44835.041569	31.926004
628.135414	44907.193961	31.931021
628.974918	44986.639269	31.936039
629.356875	45060.021734	31.941056
630.225864	45147.318495	31.946074
630.823948	45223.755785	31.951092
631.272833	45301.384453	31.956109
632.283740	45366.424494	31.961127
632.859625	45441.298314	31.966144
633.861775	45504.800697	31.971162
633.980416	45566.951731	31.976180
635.280565	45639.218726	31.981197
635.646787	45705.583623	31.986215
636.156444	45772.093143	31.991232
637.117361	45828.296489	31.996250
637.720934	45899.558630	32.001268
638.225730	45960.472783	32.006285
638.972251	46021.509562	32.011303
639.482161	46081.479990	32.016320
640.304795	46142.738540	32.021338
640.749602	46214.244934	32.026356
641.440304	46278.941825	32.031373
642.236285	46343.533852	32.036391
642.726007	46413.724574	32.041408
643.316727	46478.554857	32.046426
644.084137	46547.531381	32.051444
645.148359	46603.619806	32.056461
645.960779	46652.608575	32.061479
646.446064	46723.365999	32.066496
647.136166	46789.639256	32.071514
647.626860	46849.120015	32.076532
648.107902	46923.226487	32.081549
648.494771	46983.702319	32.086567
648.715009	47066.186775	32.091584
649.352829	47134.460551	32.096602
650.100551	47217.259277	32.101620
650.531658	47297.840225	32.106637
651.100734	47380.074984	32.111655
651.647563	47458.331786	32.116672
652.342820	47534.142087	32.121690
653.184384	47624.314176	32.126708
654.096596	47703.226974	32.131725
654.816715	47774.137385	32.136743
655.296737	47860.957398	32.141760
656.349347	47927.372842	32.146778
656.942687	48008.107895	32.151796
657.415652	48084.624877	32.156813
658.094714	48155.981948	32.161831
659.027357	48241.687346	32.166848
659.770901	48310.516800	32.171866
660.001629	48394.444628	32.176884
660.601067	48464.733324	32.181901
661.456825	48543.993334	32.186919
661.879026	48635.041973	32.191936
662.949360	48695.080366	32.196954
663.305834	48787.471844	32.201972
663.537641	48869.158217	32.206989
664.322732	48958.503583	32.212007
664.688329	49050.055614	32.217024
665.776236	49129.852425	32.222042
666.151855	49226.001349	32.227060
666.533658	49305.368617	32.232077
667.891464	49385.959826	32.237095
668.343527	49472.587060	32.242112
668.889430	49541.862979	32.247130
669.505979	49617.192980	32.252148
670.175351	49695.301295	32.257165
671.132017	49781.212257	32.262183
671.557724	49854.027051	32.267200
672.273286	49933.236684	32.272218
672.569994	50016.732484	32.277236
673.146844	50106.511221	32.282253
674.278658	50171.189983	32.287271
675.186460	50248.991372	32.292288
675.935228	50331.069181	32.297306
676.945641	50411.010299	32.302324
677.640667	50491.718344	32.307341
678.611924	50556.228408	32.312359
678.664199	50638.677288	32.317376
679.252386	50699.581841	32.322394
679.675553	50797.303235	32.327412
680.056855	50880.587625	32.332429
680.875485	50957.598402	32.337447
681.487896	51054.126563	32.342464
682.260336	51126.973386	32.347482
683.095559	51220.891785	32.352500
684.561503	51302.932455	32.357517
685.202172	51379.541019	32.362535
686.291648	51443.637815	32.367552
687.417609	51503.768339	32.372570
687.823653	51581.743766	32.377588
688.257494	51659.633051	32.382605
689.203955	51714.247839	32.387623
689.627804	51795.541436	32.392640
690.216076	51869.376854	32.397658
690.652524	51945.184002	32.402676
690.963220	52033.521963	32.407693
692.029797	52109.522995	32.412711
692.404581	52184.823378	32.417728
693.403954	52250.793156	32.422746
694.547257	52336.664565	32.427764
695.556927	52385.205349	32.432781
696.661894	52458.727374	32.437799
697.147389	52533.812754	32.442816
697.884686	52591.446030	32.447834
698.737435	52650.939009	32.452852
699.368487	52708.236085	32.457869
700.185190	52780.328239	32.462887
700.270211	52850.892799	32.467904
701.203739	52915.969675	32.472922
701.653808	52987.890622	32.477940
701.944922	53053.404820	32.482957
702.663018	53132.757561	32.487975
702.856989	53213.800609	32.492992
703.380388	53295.160855	32.498010
704.145249	53386.500992	32.503028
704.320580	53492.081872	32.508045
705.096928	53570.972753	32.513063
705.832762	53658.095760	32.518080
706.320872	53745.965638	32.523098
707.297068	53824.352357	32.528116
707.534527	53921.113351	32.533133
708.408452	54002.405182	32.538151
709.353537	54095.809710	32.543168
710.034931	54175.823067	32.548186
710.845082	54268.460864	32.553204
711.452368	54350.118650	32.558221
712.634414	54428.235316	32.563239
713.031367	54514.557821	32.568256
713.952167	54599.067597	32.573274
715.014674	54679.682201	32.578292
715.470817	54772.154803	32.583309
716.581664	54846.313721	32.588327
716.921962	54931.949630	32.593344
717.522955	55021.335447	32.598362
718.334575	55106.878206	32.603380
718.923234	55198.271265	32.608397
719.917764	55268.814045	32.613415
720.575559	55366.746856	32.618432
721.168555	55455.911951	32.623450
721.938882	55532.343808	32.628468
722.540752	55622.913004	32.633485
723.277644	55707.359327	32.638503
723.921862	55811.054424	32.643520
724.501657	55893.045460	32.648538
725.256863	55990.565197	32.653556
726.054227	56092.223523	32.658573
726.798856	56184.764661	32.663591
727.264839	56283.421069	32.668608
727.797457	56389.930931	32.673626
728.924163	56467.433766	32.678644
729.971725	56564.707976	32.683661
730.657603	56652.326729	32.688679
731.512093	56738.586873	32.693696
732.275980	56831.058746	32.698714
733.240745	56916.569780	32.703732
733.801414	57008.443519	32.708749
734.988549	57087.830323	32.713767
735.780107	57176.744859	32.718784
736.373020	57255.024190	32.723802
737.709824	57317.899545	32.728820
738.668518	57403.398020	32.733837
739.570443	57474.137647	32.738855
740.301617	57535.872623	32.743872
741.010784	57613.026868	32.748890
741.819772	57672.498982	32.753908
742.298485	57748.869659	32.758925
743.033409	57817.313625	32.763943
743.469313	57894.247351	32.768960
743.823541	57974.979698	32.773978
744.947641	58039.337300	32.778996
745.578585	58137.355415	32.784013
745.848348	58211.895428	32.789031
746.457862	58288.594787	32.794048
746.895515	58369.700739	32.799066
747.961776	58448.152867	32.804084
748.799047	58524.204463	32.809101
749.693644	58590.700012	32.814119
750.559310	58675.688770	32.819136
750.931520	58760.128183	32.824154
751.744411	58829.245425	32.829172
752.289020	58928.272814	32.834189
752.995509	59022.577009	32.839207
753.855759	59109.005146	32.844224
754.429332	59202.501054	32.849242
755.261901	59280.798146	32.854260
755.781882	59365.219937	32.859277
756.246379	59450.231884	32.864295
757.349328	59552.372058	32.869312
757.732241	59647.220300	32.874330
758.702035	59730.981725	32.879348
759.251060	59837.590868	32.884365
759.879967	59925.208891	32.889383
761.280932	60023.591130	32.894400
761.684161	60117.361850	32.899418
762.900114	60202.346014	32.904436
763.460219	60303.948374	32.909453
764.342919	60392.961668	32.914471
765.448275	60484.147020	32.919488
766.263084	60565.966591	32.924506
767.682383	60634.823495	32.929524
768.126611	60728.353933	32.934541
769.083330	60811.023460	32.939559
769.669755	60888.870733	32.944576
770.206910	60973.963285	32.949594
771.264801	61062.310888	32.954612
771.655575	61154.598399	32.959629
772.468923	61234.365529	32.964647
773.009175	61325.916470	32.969664
773.640762	61433.086748	32.974682
775.072265	61512.030410	32.979700
775.437907	61606.543960	32.984717
775.910561	61696.013928	32.989735
776.763030	61785.821737	32.994752
777.196806	61885.346566	32.999770
778.425570	61976.510042	33.004788
778.831894	62074.344539	33.009805
780.003737	62181.268874	33.014823
780.644827	62259.252047	33.019840
781.279431	62366.243990	33.024858
782.369374	62469.879947	33.029876
783.108067	62570.092458	33.034893
783.788817	62657.904420	33.039911
784.800903	62747.176664	33.044928
785.875071	62835.795244	33.049946
787.303264	62910.071645	33.054964
787.797767	62997.437984	33.059981
788.455299	63071.603994	33.064999
789.807760	63146.237587	33.070016
790.232696	63224.593876	33.075034
790.973188	63296.792802	33.080052
791.475582	63369.753070	33.085069
792.351079	63445.865888	33.090087
792.919850	63527.750089	33.095104
793.404826	63611.031180	33.100122
794.360202	63683.664759	33.105140
794.577826	63773.055641	33.110157
795.055138	63857.444337	33.115175
795.668332	63949.981654	33.120192
796.236513	64058.146385	33.125210
797.119802	64150.960654	33.130228
797.875633	64263.079024	33.135245
798.585314	64357.289385	33.140263
799.625302	64461.383132	33.145280
800.707068	64559.100804	33.150298
801.838687	64649.964137	33.155316
802.663807	64754.267376	33.160333
803.550889	64861.201577	33.165351
804.159883	64952.127415	33.170368
805.122264	65056.340973	33.175386
806.010658	65149.560373	33.180404
806.913918	65235.112756	33.185421
807.864787	65333.294213	33.190439
808.884332	65429.507100	33.195456
809.323952	65528.408896	33.200474
810.166757	65610.943757	33.205492
811.008335	65717.618358	33.210509
811.978131	65811.298610	33.215527
813.112087	65898.159535	33.220544
813.473338	65998.279557	33.225562
814.545123	66092.747179	33.230580
815.490778	66179.121362	33.235597
816.072011	66285.600504	33.240615
816.928268	66375.047158	33.245632
817.469144	66472.772219	33.250650
818.244060	66567.927426	33.255668
819.060069	66674.453468	33.260685
819.533265	66779.461715	33.265703
820.578486	66889.508952	33.270720
821.145161	66997.049280	33.275738
821.609577	67111.043642	33.280756
822.632546	67223.282049	33.285773
823.473786	67340.502721	33.290791
824.517322	67442.018814	33.295808
824.816539	67551.424148	33.300826
825.962482	67656.191099	33.305844
826.639126	67779.675810	33.310861
827.221421	67892.057706	33.315879
828.325871	67991.665444	33.320896
829.559849	68107.261521	33.325914
830.472665	68208.303344	33.330932
831.483129	68315.470788	33.335949
832.298287	68428.374665	33.340967
833.011692	68514.780428	33.345984
833.478118	68610.955020	33.351002
834.873274	68707.032827	33.356020
835.576411	68795.406259	33.361037
836.133815	68889.880924	33.366055
837.555859	68981.154341	33.371072
837.965591	69077.245484	33.376090
838.965504	69162.130159	33.381108
839.976816	69268.740420	33.386125
840.741828	69368.605064	33.391143
841.525073	69460.032919	33.396160
841.618860	69560.851958	33.401178
842.645293	69666.242616	33.406196
843.364093	69781.077663	33.411213
844.018840	69888.392473	33.416231
845.131025	69989.506547	33.421248
845.603689	70108.483104	33.426266
846.255372	70222.314194	33.431284
847.290776	70327.169929	33.436301
848.266235	70451.698045	33.441319
849.153280	70564.154196	33.446336
850.303323	70677.289422	33.451354
850.903112	70780.675230	33.456372
851.926009	70902.064756	33.461389
852.304039	71020.278398	33.466407
853.523869	71137.259380	33.471424
854.120375	71256.166286	33.476442
855.057601	71381.154964	33.481460
856.190520	71495.567626	33.486477
857.096107	71606.630362	33.491495
857.791695	71716.545557	33.496512
858.965072	71841.486925	33.501530
859.793292	71964.594713	33.506548
861.012186	72069.493687	33.511565
861.429089	72178.988204	33.516583
862.758022	72296.047135	33.521600
863.411768	72415.564807	33.526618
864.501755	72517.162947	33.531636
865.336873	72628.021452	33.536653
865.876381	72739.926007	33.541671
866.691398	72852.166488	33.546688
867.730656	72973.730386	33.551706
868.527633	73090.423669	33.556724
869.257391	73201.276851	33.561741
870.088898	73321.371980	33.566759
871.197735	73435.350982	33.571776
871.903883	73562.816701	33.576794
872.547836	73699.108479	33.581812
873.782700	73810.952619	33.586829
873.941820	73916.206889	33.591847
874.621786	74030.756751	33.596864
875.612878	74165.366067	33.601882
876.343866	74286.803733	33.606900
877.567920	74421.895893	33.611917
878.201942	74559.048220	33.616935
879.628543	74659.630481	33.621952
880.166905	74778.946804	33.626970
881.088985	74904.914220	33.631988
881.940050	75020.883373	33.637005
882.679150	75131.947962	33.642023
883.879655	75253.297791	33.647040
884.726060	75372.644449	33.652058
885.589328	75488.115084	33.657076
886.629146	75596.081910	33.662093
887.460858	75730.290976	33.667111
888.322435	75858.877765	33.672128
889.827346	75962.316996	33.677146
890.688870	76074.296319	33.682164
891.968674	76185.185861	33.687181
892.863196	76299.809272	33.692199
893.848862	76393.966999	33.697216
894.820988	76499.983869	33.702234
895.415658	76609.619601	33.707252
896.246613	76712.259796	33.712269
897.023727	76830.248264	33.717287
897.987964	76946.400047	33.722304
898.755212	77058.304993	33.727322
899.389851	77164.985778	33.732340
900.484380	77278.148166	33.737357
901.252998	77389.858783	33.742375
901.971672	77509.149843	33.747392
903.024325	77631.934246	33.752410
904.107080	77755.555226	33.757428
905.243516	77864.719635	33.762445
905.739052	77990.913126	33.767463
906.843764	78104.830626	33.772480
907.744865	78213.370674	33.777498
908.602821	78335.905852	33.782516
909.582330	78463.731837	33.787533
910.483076	78584.605661	33.792551
911.316060	78704.144646	33.797568
912.050819	78818.352522	33.802586
912.868399	78942.054456	33.807604
913.898977	79066.854688	33.812621
914.809180	79193.880844	33.817639
915.451323	79316.569983	33.822656
916.832323	79441.082853	33.827674
917.597298	79570.239338	33.832692
918.306553	79703.956698	33.837709
919.068456	79832.211391	33.842727
920.451020	79948.844602	33.847744
921.606158	80067.676515	33.852762
922.323486	80194.151639	33.857780
923.278428	80311.695662	33.862797
924.182614	80439.899878	33.867815
925.009981	80565.000670	33.872832
925.892394	80686.585075	33.877850
926.727023	80819.897764	33.882868
928.024024	80942.460746	33.887885
928.885938	81064.177052	33.892903
930.228562	81165.329411	33.897920
931.064920	81273.775743	33.902938
931.458079	81385.593040	33.907956
933.038883	81488.163049	33.912973
933.721254	81602.072214	33.917991
934.669219	81707.411741	33.923008
935.637572	81810.358933	33.928026
936.141507	81927.130406	33.933044
937.283947	82027.035478	33.938061
937.880689	82154.919861	33.943079
938.501575	82287.719619	33.948096
939.762254	82408.533193	33.953114
940.507842	82530.757026	33.958132
941.513869	82653.483830	33.963149
942.374208	82787.645823	33.968167
943.211868	82912.828596	33.973184
944.405553	83037.993407	33.978202
945.379210	83157.794845	33.983220
946.499083	83283.971765	33.988237
947.395268	83397.319286	33.993255
948.467423	83523.366145	33.998272
949.914751	83647.659693	34.003290
950.436583	83772.714481	34.008308
951.451834	83889.023528	34.013325
952.703215	84006.787740	34.018343
953.305259	84131.098488	34.023360
954.442618	84229.035918	34.028378
955.276750	84368.364967	34.033396
956.120008	84500.688082	34.038413
956.680398	84614.436977	34.043431
957.731146	84744.553633	34.048448
958.805490	84858.133553	34.053466
959.550997	85003.582250	34.058484
960.694269	85131.049987	34.063501
961.655773	85270.086494	34.068519
962.082309	85406.445938	34.073536
964.019748	85529.800021	34.078554
964.543598	85658.709909	34.083572
965.529546	85794.824771	34.088589
966.554222	85941.025828	34.093607
967.595749	86070.380656	34.098624
969.172534	86200.801916	34.103642
969.772910	86335.824444	34.108660
970.875177	86441.947108	34.113677
972.023261	86571.578883	34.118695
972.880820	86694.807984	34.123712
974.203329	86816.016269	34.128730
975.150677	86945.694887	34.133748
975.930802	87056.816654	34.138765
976.724027	87191.459786	34.143783
977.478549	87317.231871	34.148800
978.449335	87455.421126	34.153818
978.826705	87588.324392	34.158836
979.911931	87727.205415	34.163853
980.930637	87859.104065	34.168871
982.068107	87983.902208	34.173888
983.201311	88107.746885	34.178906
984.066747	88234.031535	34.183924
984.730337	88352.691034	34.188941
985.633826	88490.100836	34.193959
986.653913	88619.360586	34.198976
987.718053	88751.889835	34.203994
988.418252	88890.694135	34.209012
989.238125	89017.926535	34.214029
990.227757	89158.065111	34.219047
991.158545	89311.791524	34.224064
992.187101	89445.639732	34.229082
992.830263	89581.074165	34.234100
993.740309	89727.850358	34.239117
995.019134	89877.180745	34.244135
996.169993	90016.590898	34.249152
997.840091	90154.262400	34.254170
998.602765	90310.640827	34.259188
999.565460	90446.485149	34.264205
1000.475353	90579.941787	34.269223
1001.184000	90728.989235	34.274240
1002.418257	90882.773302	34.279258
1003.437680	91038.040927	34.284276
1004.558582	91177.735194	34.289293
1005.447012	91323.323868	34.294311
1006.567186	91474.062814	34.299328
1007.486450	91618.807367	34.304346
1008.482282	91770.852026	34.309364
1009.558727	91917.255903	34.314381
1010.350778	92070.758107	34.319399
1010.867496	92231.256147	34.324416
1012.077437	92382.998997	34.329434
1012.984629	92552.298385	34.334452
1014.050780	92711.883951	34.339469
1015.481441	92850.843797	34.344487
1016.386286	93023.119902	34.349504
1018.079613	93162.577551	34.354522
1019.517018	93303.164706	34.359540
1020.632964	93435.106786	34.364557
1022.035026	93569.799877	34.369575
1023.188939	93714.274121	34.374592
1024.018437	93845.884685	34.379610
1024.968141	93976.319373	34.384628
1026.232920	94110.259556	34.389645
1027.204543	94234.778066	34.394663
1027.955439	94363.443903	34.399680
1028.938776	94501.840019	34.404698
1029.628772	94654.629889	34.409716
1030.503363	94801.647843	34.414733
1031.458431	94946.345120	34.419751
1032.233103	95099.143525	34.424768
1033.204801	95246.553787	34.429786
1034.225855	95406.576966	34.434804
1035.013602	95551.987933	34.439821
1035.964770	95706.989060	34.444839
1036.995128	95855.431411	34.449856
1038.035309	95995.200390	34.454874
1039.149054	96134.458787	34.459892
1040.375900	96268.462161	34.464909
1041.943245	96398.502708	34.469927
1043.394850	96537.216424	34.474944
1044.383770	96662.390879	34.479962
1045.493266	96807.556320	34.484980
1046.581001	96933.646496	34.489997
1047.690050	97045.430498	34.495015
1048.363033	97199.379017	34.500032
1049.278343	97330.781214	34.505050
1050.146214	97462.792713	34.510068
1050.863610	97607.734621	34.515085
1051.907724	97752.884867	34.520103
1052.689598	97911.097504	34.525120
1053.764564	98067.790556	34.530138
1054.583033	98221.400187	34.535156
1055.946585	98367.933327	34.540173
1057.288729	98519.652283	34.545191
1057.673607	98686.860235	34.550208
1058.813556	98845.579125	34.555226
1060.277831	99001.356222	34.560244
1060.982274	99156.103754	34.565261
1062.297124	99310.831167	34.570279
1063.169577	99476.341328	34.575296
1064.368010	99635.790288	34.580314
1065.718454	99799.872798	34.585332
1066.593655	99948.239924	34.590349
1068.116579	100114.480047	34.595367
1068.629989	100278.553559	34.600384
1070.131872	100433.322028	34.605402
1071.075822	100599.075619	34.610420
1072.041381	100749.458200	34.615437
1073.308421	100911.100580	34.620455
1074.583348	101075.691345	34.625472
1075.524360	101231.073175	34.630490
1076.658075	101384.002014	34.635508
1077.740698	101549.885863	34.640525
1078.843348	101712.097783	34.645543
1079.522035	101875.669065	34.650560
1080.996858	102034.445152	34.655578
1082.161815	102187.235082	34.660596
1083.017198	102350.319670	34.665613
1084.367246	102502.303923	34.670631
1085.298863	102672.041662	34.675648
1086.315432	102839.552402	34.680666
1087.675450	102990.127140	34.685684
1088.882302	103142.157294	34.690701
1090.172613	103296.092507	34.695719
1090.815808	103457.123994	34.700736
1092.050617	103624.504367	34.705754
1093.206730	103779.077889	34.710772
1094.019980	103948.463972	34.715789
1095.457047	104090.933581	34.720807
1096.352648	104237.255397	34.725824
1097.371719	104378.179535	34.730842
1098.669434	104530.957235	34.735860
1099.561140	104674.535926	34.740877
1100.820114	104817.221746	34.745895
1101.437093	104970.325690	34.750912
1102.538195	105114.759707	34.755930
1103.444367	105284.830342	34.760948
1104.360741	105446.274881	34.765965
1105.776878	105608.862438	34.770983
1106.933455	105771.618950	34.776000
1107.929156	105919.567957	34.781018
1109.036101	106085.625361	34.786036
1109.712284	106243.347948	34.791053
1110.939978	106412.508448	34.796071
1112.133434	106582.093283	34.801088
1113.503229	106751.784179	34.806106
1114.668706	106919.154434	34.811124
1115.534551	107094.661820	34.816141
1116.862207	107255.084816	34.821159
1117.800833	107420.184565	34.826176
1119.040739	107592.053887	34.831194
1120.095672	107775.681605	34.836212
1121.885152	107932.877462	34.841229
1123.134101	108083.666588	34.846247
1124.414540	108241.337802	34.851264
1125.480005	108414.664772	34.856282
1126.730565	108563.690770	34.861300
1127.791126	108715.950527	34.866317
1129.152412	108877.100464	34.871335
1130.083653	109032.452502	34.876352
1131.225666	109190.968379	34.881370
1132.447378	109358.365530	34.886388
1133.024581	109527.967714	34.891405
1134.861513	109691.079173	34.896423
1135.487454	109843.915113	34.901440
1136.420166	110017.584731	34.906458
1137.864768	110182.274633	34.911476
1138.721003	110358.965430	34.916493
1139.570275	110533.810307	34.921511
1140.893146	110693.205973	34.926528
1141.896733	110870.579623	34.931546
1143.399785	111033.025154	34.936564
1144.166567	111221.883464	34.941581
1145.679250	111396.451729	34.946599
1146.887984	111568.233696	34.951616
1148.014740	111729.642213	34.956634
1149.616375	111890.463532	34.961652
1150.894466	112059.566562	34.966669
1151.981222	112223.953507	34.971687
1152.978009	112396.889030	34.976704
1153.627332	112568.418703	34.981722
1154.972748	112734.831571	34.986740
1155.953068	112913.527579	34.991757
1157.520216	113079.616294	34.996775
1158.323679	113238.477861	35.001792
1159.360997	113391.650108	35.006810
1160.718683	113545.152185	35.011828
1161.639671	113719.526957	35.016845
1163.145891	113874.444478	35.021863
1164.106960	114027.822652	35.026880
1164.969318	114183.749740	35.031898
1166.116385	114345.045316	35.036916
1167.019750	114526.335331	35.041933
1168.321539	114700.143556	35.046951
1169.302683	114861.012991	35.051968
1170.308918	115043.436250	35.056986
1171.772439	115208.618531	35.062004
1172.784059	115392.221005	35.067021
1174.352259	115565.112802	35.072039
1175.933772	115724.689365	35.077056
1177.144790	115896.582917	35.082074
1178.348285	116057.557544	35.087092
1179.572406	116228.248328	35.092109
1180.816594	116389.649106	35.097127
1182.069343	116565.396272	35.102144
1182.976481	116729.372643	35.107162
1184.066038	116904.236371	35.112180
1185.148261	117096.431587	35.117197
1186.150896	117259.699711	35.122215
1187.219308	117444.928780	35.127232
1188.024851	117628.877680	35.132250
1189.279541	117802.423298	35.137268
1190.539889	118006.506754	35.142285
1191.936994	118198.235917	35.147303
1193.343798	118366.607141	35.152320
1194.292911	118554.611127	35.157338
1195.807836	118748.459453	35.162356
1197.007707	118923.901877	35.167373
1198.012685	119115.421573	35.172391
1199.571556	119306.050460	35.177408
1200.611199	119486.657389	35.182426
1201.578331	119675.375808	35.187444
1202.500582	119875.639834	35.192461
1203.996601	120054.234179	35.197479
1205.195790	120244.490191	35.202496
1206.014486	120458.351387	35.207514
1207.508215	120640.483494	35.212532
1208.778042	120855.327366	35.217549
1209.670954	121034.353555	35.222567
1211.038687	121234.316503	35.227584
1212.419233	121439.712209	35.232602
1214.051780	121633.189610	35.237620
1214.970746	121821.829794	35.242637
1216.246082	122015.417443	35.247655
1217.439645	122214.389616	35.252672
1218.466399	122416.011547	35.257690
1219.863079	122593.372358	35.262708
1220.878776	122801.230411	35.267725
1222.298064	122980.996683	35.272743
1223.302302	123165.909137	35.277760
1224.450232	123349.723428	35.282778
1225.964354	123524.893237	35.287796
1227.111950	123717.322972	35.292813
1228.440987	123902.986851	35.297831
1229.627257	124075.957811	35.302848
1230.132336	124273.699500	35.307866
1231.612982	124451.907941	35.312884
1233.087033	124646.965053	35.317901
1234.273356	124829.238062	35.322919
1235.436597	125027.881316	35.327936
1236.401374	125219.996192	35.332954
1237.611501	125410.325403	35.337972
1238.812200	125614.958436	35.342989
1240.047903	125816.851365	35.348007
1241.515137	126019.291677	35.353024
1242.706667	126215.532377	35.358042
1244.453503	126407.797348	35.363060
1245.802450	126596.491380	35.368077
1247.036215	126799.569971	35.373095
1248.492660	126996.141530	35.378112
1249.388250	127187.103198	35.383130
1250.887579	127388.269122	35.388148
1251.523519	127600.822836	35.393165
1253.050352	127787.672619	35.398183
1254.563958	127987.763884	35.403200
1256.035820	128194.019956	35.408218
1257.169785	128392.033584	35.413236
1258.328180	128589.677366	35.418253
1259.504122	128784.963443	35.423271
1260.655741	128994.772872	35.428288
1261.900033	129208.217714	35.433306
1263.153009	129413.491500	35.438324
1264.721156	129606.884048	35.443341
1265.674629	129815.882354	35.448359
1267.277801	130023.930129	35.453376
1268.106328	130237.258899	35.458394
1268.899943	130453.825481	35.463412
1270.455066	130654.651482	35.468429
1271.566609	130889.959414	35.473447
1272.901547	131100.971769	35.478464
1274.530197	131324.583240	35.483482
1275.664550	131530.980967	35.488500
1276.761251	131756.568191	35.493517
1278.097767	131969.626616	35.498535
1279.870775	132180.767449	35.503552
1281.121490	132392.867105	35.508570
1282.537372	132595.654882	35.513588
1283.571868	132813.759675	35.518605
1284.847397	133033.031503	35.523623
1286.420928	133243.540398	35.528640
1287.677197	133464.098306	35.533658
1288.972173	133672.602009	35.538676
1290.347038	133878.066231	35.543693
1291.595165	134086.187591	35.548711
1292.887963	134281.290363	35.553728
1293.908726	134489.298723	35.558746
1295.182609	134681.429531	35.563764
1296.283379	134885.614041	35.568781
1297.156119	135083.209182	35.573799
1298.354422	135285.581693	35.578816
1299.825689	135512.203320	35.583834
1301.348118	135716.605429	35.588852
1302.381347	135915.777330	35.593869
1303.390646	136147.495275	35.598887
1305.057288	136358.278164	35.603904
1306.467068	136575.097193	35.608922
1307.724676	136780.296477	35.613940
1309.112465	136989.493545	35.618957
1310.373005	137211.409817	35.623975
1311.987241	137427.214213	35.628992
1313.011510	137646.941002	35.634010
1314.887735	137859.614873	35.639028
1315.817669	138078.840295	35.644045
1316.787655	138308.199065	35.649063
1318.609752	138510.431304	35.654080
1320.069903	138728.816894	35.659098
1321.268664	138953.835532	35.664116
1322.608303	139175.982056	35.669133
1323.775704	139398.867298	35.674151
1325.387754	139613.293890	35.679168
1326.183719	139848.673895	35.684186
1327.666434	140075.252667	35.689204
1328.969484	140291.456790	35.694221
1330.104506	140526.851580	35.699239
1331.683521	140752.951223	35.704256
1333.036554	140986.046359	35.709274
1334.536421	141210.996020	35.714292
1336.087156	141422.885114	35.719309
1337.339511	141656.406968	35.724327
1338.999653	141877.762019	35.729344
1340.171603	142107.054276	35.734362
1341.560123	142322.562212	35.739380
1343.641459	142550.661308	35.744397
1345.183402	142761.141564	35.749415
1346.806452	142956.857177	35.754432
1348.167553	143165.569157	35.759450
1349.264552	143379.964783	35.764468
1350.673601	143591.866066	35.769485
1351.897434	143796.155266	35.774503
1353.377630	143999.086874	35.779520
1354.361963	144219.007170	35.784538
1355.495315	144439.298271	35.789556
1357.102067	144658.058046	35.794573
1358.129866	144879.890071	35.799591
1359.415701	145092.873236	35.804608
1360.678869	145315.989200	35.809626
1361.970049	145547.632995	35.814644
1363.465407	145761.956383	35.819661
1364.521768	145987.822592	35.824679
1366.107424	146194.617833	35.829696
1367.157419	146412.768489	35.834714
1368.471813	146624.261734	35.839732
1369.772570	146840.283943	35.844749
1370.888323	147071.941464	35.849767
1372.506368	147276.393530	35.854784
1373.661542	147498.071635	35.859802
1374.828539	147726.708799	35.864820
1376.216185	147954.108262	35.869837
1377.250834	148183.847238	35.874855
1378.655943	148410.309095	35.879872
1380.285062	148647.854556	35.884890
1381.686965	148871.150958	35.889908
1383.171716	149103.170222	35.894925
1384.220324	149347.278381	35.899943
1385.540184	149572.532276	35.904960
1386.758510	149806.234285	35.909978
1388.310340	150060.384350	35.914996
1390.217580	150318.587439	35.920013
1391.030372	150555.921658	35.925031
1392.588672	150794.761884	35.930048
1393.814175	151056.235886	35.935066
1395.359133	151300.431952	35.940084
1396.606477	151548.125537	35.945101
1397.999908	151805.065453	35.950119
1399.308337	152057.824399	35.955136
1401.062778	152312.264010	35.960154
1402.688057	152551.752941	35.965172
1404.659200	152787.448498	35.970189
1407.230786	153011.538198	35.975207
1409.412075	153216.711520	35.980224
1411.263667	153426.109787	35.985242
1412.877954	153626.519782	35.990260
1414.725726	153831.838634	35.995277
1415.803862	154030.409051	36.000295
1416.862324	154235.183804	36.005312
1418.309604	154437.628466	36.010330
1419.456260	154646.804032	36.015348
1420.636211	154855.899527	36.020365
1421.822369	155063.689359	36.025383
1423.110480	155277.398225	36.030400
1424.610750	155492.913253	36.035418
1425.950491	155715.466951	36.040436
1427.627649	155929.701364	36.045453
1428.927995	156139.888764	36.050471
1430.140278	156354.846373	36.055488
1431.714878	156573.501010	36.060506
1432.752683	156800.471626	36.065524
1433.994029	157016.214919	36.070541
1435.038179	157249.768432	36.075559
1436.517803	157475.658888	36.080576
1438.028575	157709.711982	36.085594
1439.111705	157953.268811	36.090612
1440.531678	158186.933780	36.095629
1442.072405	158418.577605	36.100647
1443.114269	158648.869317	36.105664
1444.658230	158865.717293	36.110682
1445.728620	159103.184753	36.115700
1447.160513	159321.397521	36.120717
1448.481225	159558.879016	36.125735
1450.090037	159778.917937	36.130752
1451.806174	160019.788960	36.135770
1452.551561	160263.580361	36.140788
1454.294908	160495.611490	36.145805
1455.828211	160731.938454	36.150823
1456.974945	160975.138357	36.155840
1458.370352	161222.104880	36.160858
1459.888296	161463.752712	36.165876
1461.512913	161712.309456	36.170893
1462.586482	161968.830883	36.175911
1464.087638	162221.075810	36.180928
1465.732145	162468.810300	36.185946
1466.937156	162734.548791	36.190964
1468.356160	162993.203938	36.195981
1469.715521	163265.148749	36.200999
1471.119444	163518.103002	36.206016
1472.514529	163791.314302	36.211034
1474.163089	164066.668776	36.216052
1476.126673	164328.658487	36.221069
1477.399659	164599.155755	36.226087
1479.105620	164860.403853	36.231104
1480.731913	165124.862554	36.236122
1482.033583	165399.863569	36.241140
1483.556004	165652.610750	36.246157
1484.880387	165938.024970	36.251175
1486.557542	166202.039349	36.256192
1488.243556	166465.102933	36.261210
1489.761472	166720.445471	36.266228
1491.559547	166990.420111	36.271245
1493.034338	167260.169005	36.276263
1494.775630	167526.693873	36.281280
1496.570544	167779.183792	36.286298
1497.813925	168048.860916	36.291316
1499.289319	168301.024547	36.296333
1500.779305	168561.584390	36.301351
1502.043601	168831.986724	36.306368
1503.753804	169087.974236	36.311386
1505.226333	169350.191169	36.316404
1506.915444	169615.191427	36.321421
1508.417328	169875.288971	36.326439
1509.665893	170147.884782	36.331456
1511.650564	170403.697895	36.336474
1512.628295	170684.243052	36.341492
1514.699857	170939.107209	36.346509
1516.086198	171213.312254	36.351527
1517.601846	171476.995468	36.356544
1519.060604	171734.220078	36.361562
1520.185339	172004.882315	36.366580
1521.632889	172261.718904	36.371597
1523.418831	172542.110884	36.376615
1524.858101	172789.159097	36.381632
1526.726025	173028.770460	36.386650
1528.056502	173283.323483	36.391668
1529.645039	173528.259439	36.396685
1530.894015	173769.483156	36.401703
1532.328176	174031.255345	36.406720
1533.654319	174279.409020	36.411738
1534.787387	174548.869322	36.416756
1536.416736	174798.677947	36.421773
1538.130509	175071.791879	36.426791
1539.554982	175317.893817	36.431808
1541.766548	175571.636251	36.436826
1543.303394	175837.932800	36.441844
1544.773090	176105.205916	36.446861
1546.821199	176346.673215	36.451879
1548.283560	176611.438842	36.456896
1550.405327	176853.392188	36.461914
1551.708330	177114.519883	36.466932
1553.567176	177353.587257	36.471949
1555.206307	177611.366094	36.476967
1556.755207	177852.819960	36.481984
1558.639412	178096.518327	36.487002
1559.815198	178342.081459	36.492020
1561.442550	178598.548772	36.497037
1563.519048	178842.855283	36.502055
1564.499428	179099.555268	36.507072
1565.954010	179350.928873	36.512090
1567.409937	179606.516017	36.517108
1568.997025	179862.540615	36.522125
1570.159952	180124.013701	36.527143
1571.683511	180399.806362	36.532160
1573.246590	180662.424510	36.537178
1574.415966	180940.332319	36.542196
1576.128847	181210.035253	36.547213
1577.902499	181491.631656	36.552231
1578.865593	181759.782256	36.557248
1580.791474	182039.822754	36.562266
1582.276714	182311.027808	36.567284
1583.700206	182593.042193	36.572301
1585.682222	182878.395576	36.577319
1587.186968	183167.442850	36.582336
1589.126999	183437.453317	36.587354
1590.551936	183716.162890	36.592372
1591.958474	183991.032413	36.597389
1594.263891	184263.997110	36.602407
1595.527947	184547.546509	36.607424
1597.669654	184817.812443	36.612442
1599.123404	185100.332758	36.617460
1600.799984	185367.072133	36.622477
1602.337835	185641.740533	36.627495
1603.713349	185915.903417	36.632512
1605.599072	186193.286173	36.637530
1607.250510	186483.942985	36.642548
1608.634412	186754.201178	36.647565
1610.374636	187022.450158	36.652583
1611.577523	187289.390157	36.657600
1613.043327	187545.199040	36.662618
1614.561484	187798.907184	36.667636
1616.512061	188052.992185	36.672653
1618.136283	188301.699066	36.677671
1619.332335	188576.629530	36.682688
1621.314612	188829.495453	36.687706
1622.584332	189097.450357	36.692724
1624.102899	189361.306362	36.697741
1626.086297	189631.270226	36.702759
1627.478305	189900.174703	36.707776
1628.796292	190181.643368	36.712794
1630.160757	190463.068230	36.717812
1631.505496	190746.388777	36.722829
1633.356729	191035.607894	36.727847
1634.667171	191324.876541	36.732864
1636.164541	191616.109694	36.737882
1637.710855	191907.933287	36.742900
1639.267451	192216.585313	36.747917
1640.613583	192517.886460	36.752935
1642.536316	192834.733450	36.757952
1644.176979	193132.552254	36.762970
1646.116277	193451.164636	36.767988
1647.532313	193768.098032	36.773005
1649.351453	194066.477873	36.778023
1650.633234	194397.587606	36.783040
1652.690978	194705.033218	36.788058
1654.103879	195021.860765	36.793076
1655.558109	195337.122624	36.798093
1657.544323	195656.553746	36.803111
1659.187877	195976.472795	36.808128
1660.825997	196292.828220	36.813146
1662.386061	196616.635574	36.818164
1664.204219	196928.067116	36.823181
1666.286052	197256.047494	36.828199
1667.963295	197589.259971	36.833216
1669.695081	197909.621121	36.838234
1671.729090	198213.677082	36.843252
1673.404580	198529.735462	36.848269
1675.334013	198845.349230	36.853287
1677.004399	199158.010500	36.858304
1678.701304	199462.292110	36.863322
1680.844768	199763.927872	36.868340
1682.765919	200070.474718	36.873357
1684.531968	200367.908927	36.878375
1686.182277	200673.194786	36.883392
1688.355941	200964.157496	36.888410
1690.095255	201254.264104	36.893428
1691.435579	201562.168151	36.898445
1693.261597	201857.392256	36.903463
1694.856964	202156.411810	36.908480
1696.652031	202455.629741	36.913498
1698.660395	202741.931406	36.918516
1700.118296	203023.841066	36.923533
1702.358942	203297.795831	36.928551
1704.383439	203571.011918	36.933568
1705.992205	203823.172783	36.938586
1707.658766	204071.276235	36.943604
1709.138860	204327.204443	36.948621
1711.010990	204592.845925	36.953639
1712.171048	204860.886611	36.958656
1714.103788	205115.134296	36.963674
1716.058129	205379.065314	36.968692
1717.114719	205652.559172	36.973709
1718.993787	205912.239281	36.978727
1720.210647	206193.402943	36.983744
1721.807433	206475.878619	36.988762
1723.474564	206750.245399	36.993780
1724.929727	207041.759313	36.998797
1726.583018	207323.455662	37.003815
1727.767303	207624.815630	37.008832
1729.934517	207926.693870	37.013850
1731.739584	208234.000995	37.018868
1732.994283	208526.582167	37.023885
1734.818075	208828.024291	37.028903
1736.716249	209140.183326	37.033920
1738.460707	209450.375221	37.038938
1740.332083	209752.753730	37.043956
1742.024522	210060.836844	37.048973
1743.969815	210371.572714	37.053991
1746.273238	210667.552136	37.059008
1748.844406	210948.027526	37.064026
1751.838710	211196.317669	37.069044
1754.428557	211453.648656	37.074061
1756.988987	211696.423636	37.079079
1758.843375	211959.535591	37.084096
1760.603613	212209.536335	37.089114
1762.185138	212439.926283	37.094132
1763.643826	212693.798143	37.099149
1764.882895	212935.175177	37.104167
1766.543542	213195.974178	37.109184
1768.001838	213450.521902	37.114202
1769.433382	213715.713990	37.119220
1770.766765	213998.151081	37.124237
1772.627238	214260.471450	37.129255
1773.955830	214543.990762	37.134272
1775.220752	214828.016521	37.139290
1777.053117	215113.083350	37.144308
1778.276622	215406.310102	37.149325
1780.003459	215701.121421	37.154343
1781.458075	216003.264890	37.159360
1783.408707	216305.013535	37.164378
1784.783841	216609.838501	37.169396
1786.234147	216929.825139	37.174413
1788.068494	217242.070879	37.179431
1789.643399	217564.084762	37.184448
1791.220700	217884.372984	37.189466
1793.216037	218210.893847	37.194484
1794.799732	218542.763386	37.199501
1796.694696	218872.464675	37.204519
1798.538922	219180.590844	37.209536
1800.073652	219487.015266	37.214554
1802.159953	219790.026810	37.219572
1803.575923	220110.007645	37.224589
1805.675160	220407.851978	37.229607
1807.910591	220720.721977	37.234624
1809.831302	221026.697879	37.239642
1811.553587	221330.357529	37.244660
1813.771197	221615.528720	37.249677
1815.915512	221964.427812	37.254695
1817.967969	222270.502079	37.259712
1819.557096	222577.197089	37.264730
1821.137971	222877.723641	37.269748
1822.884731	223186.326045	37.274765
1825.084675	223480.496766	37.279783
1826.780652	223785.071743	37.284800
1828.614145	224098.946157	37.289818
1830.765556	224394.473917	37.294836
1832.284630	224713.416239	37.299853
1833.867316	225029.543500	37.304871
1836.041378	225338.911742	37.309888
1837.774169	225649.684469	37.314906
1839.632925	225966.698473	37.319924
1841.259726	226293.464485	37.324941
1843.493683	226592.732981	37.329959
1845.260312	226909.777879	37.334976
1847.132419	227230.438898	37.339994
1849.190296	227535.351258	37.345012
1850.629136	227863.346785	37.350029
1852.759226	228176.808580	37.355047
1855.042657	228497.485225	37.360064
1857.110100	228812.432254	37.365082
1859.122316	229114.436768	37.370100
1860.896280	229436.315146	37.375117
1862.782099	229737.198968	37.380135
1864.648081	230051.344247	37.385152
1866.477056	230371.083878	37.390170
1868.547566	230681.059126	37.395188
1870.401991	230995.387270	37.400205
1872.243563	231298.670617	37.405223
1874.061283	231613.184459	37.410240
1876.085850	231933.711169	37.415258
1878.295828	232240.342378	37.420276
1880.055796	232546.436442	37.425293
1882.210555	232854.500663	37.430311
1884.274150	233151.659205	37.435328
1885.915766	233457.546355	37.440346
1888.093142	233761.444578	37.445364
1890.232829	234053.260172	37.450381
1892.078981	234353.809416	37.455399
1894.026909	234655.537133	37.460416
1895.999729	234953.909209	37.465434
1898.173525	235237.925513	37.470452
1900.360695	235531.058570	37.475469
1902.435530	235801.046725	37.480487
1904.243564	236071.662090	37.485504
1905.934485	236335.083489	37.490522
1907.599769	236583.727496	37.495540
1909.623460	236842.169982	37.500557
1911.438991	237095.972719	37.505575
1913.170534	237365.384377	37.510592
1915.003663	237621.928654	37.515610
1917.170752	237890.408933	37.520628
1918.647113	238180.309404	37.525645
1920.266204	238452.408499	37.530663
1921.807188	238734.934376	37.535680
1923.279160	239024.710741	37.540698
1924.848784	239318.815659	37.545716
1926.641527	239624.341116	37.550733
1928.532534	239927.667427	37.555751
1930.729483	240232.393765	37.560768
1932.140174	240554.034875	37.565786
1934.262869	240850.926082	37.570804
1936.208554	241177.055951	37.575821
1938.040063	241502.112623	37.580839
1939.762493	241816.494073	37.585856
1941.639700	242147.285609	37.590874
1943.666242	242480.899146	37.595892
1945.754384	242809.855562	37.600909
1947.529006	243140.818399	37.605927
1949.542538	243469.331154	37.610944
1951.291345	243803.297031	37.615962
1953.691862	244136.626949	37.620980
1955.574886	244480.784237	37.625997
1957.563627	244815.857629	37.631015
1959.768090	245149.322787	37.636032
1961.423296	245488.641867	37.641050
1963.667696	245832.237231	37.646068
1965.846367	246163.753074	37.651085
1968.201607	246503.700177	37.656103
1970.164698	246834.261154	37.661120
1971.965501	247171.681506	37.666138
1974.342549	247496.869501	37.671156
1976.205684	247829.836286	37.676173
1978.487621	248163.169186	37.681191
1980.657338	248481.813309	37.686208
1982.545959	248823.135235	37.691226
1984.603706	249149.850709	37.696244
1986.574452	249482.956413	37.701261
1988.266525	249807.572138	37.706279
1990.486691	250138.074084	37.711296
1992.550906	250468.931659	37.716314
1994.734170	250788.035470	37.721332
1996.713635	251121.295533	37.726349
1998.564142	251455.821389	37.731367
2000.787084	251781.779223	37.736384
2002.833190	252117.240585	37.741402
2004.750520	252438.701196	37.746420
2006.578805	252754.638897	37.751437
2008.564394	253083.913599	37.756455
2010.417212	253391.491266	37.761472
2012.220610	253704.056069	37.766490
2014.272710	253999.511754	37.771508
2016.063355	254319.623987	37.776525
2017.856358	254636.205471	37.781543
2019.653427	254942.295716	37.786560
2021.547992	255266.812958	37.791578
2023.759950	255595.065294	37.796596
2025.526550	255925.598794	37.801613
2027.431183	256260.607119	37.806631
2029.080817	256589.839272	37.811648
2030.720655	256928.955002	37.816666
2032.983053	257263.476252	37.821684
2035.701331	257610.550705	37.826701
2037.813990	257947.255908	37.831719
2040.198125	258279.269856	37.836736
2042.134352	258620.474836	37.841754
2043.930094	258955.986981	37.846772
2046.101730	259306.605324	37.851789
2048.067502	259648.162637	37.856807
2050.547923	259983.872337	37.861824
2052.261464	260342.312545	37.866842
2054.515172	260683.114211	37.871860
2056.912496	261028.745443	37.876877
2058.831137	261380.143251	37.881895
2061.137330	261720.937809	37.886912
2063.249335	262070.552951	37.891930
2065.365440	262405.891388	37.896948
2067.426461	262756.658502	37.901965
2069.412749	263093.898053	37.906983
2071.994814	263424.311643	37.912000
2074.197997	263774.752419	37.917018
2076.314454	264107.348948	37.922036
2078.775958	264445.098674	37.927053
2080.584542	264789.480853	37.932071
2082.873525	265118.240428	37.937088
2084.536402	265467.320468	37.942106
2086.517288	265813.174959	37.947124
2088.800322	266154.866484	37.952141
2090.564878	266501.213073	37.957159
2092.893178	266853.160818	37.962176
2094.828520	267210.124768	37.967194
2096.872620	267556.681785	37.972212
2099.326938	267907.822757	37.977229
2101.299816	268258.684658	37.982247
2103.419798	268605.408100	37.987264
2105.320177	268949.372197	37.992282
2107.254474	269299.478695	37.997300
2109.623451	269652.768050	38.002317
2111.677199	270012.585418	38.007335
2113.818580	270360.906732	38.012352
2115.790202	270719.035404	38.017370
2118.058575	271070.029607	38.022388
2120.437267	271420.168123	38.027405
2122.403974	271769.660793	38.032423
2124.817723	272092.434507	38.037440
2127.045072	272409.598305	38.042458
2128.898456	272726.592846	38.047476
2131.046724	273043.693099	38.052493
2132.696242	273372.177015	38.057511
2135.287419	273690.172449	38.062528
2137.107819	274014.209151	38.067546
2139.139472	274352.590709	38.072564
2141.357905	274676.157878	38.077581
2143.174860	275014.929163	38.082599
2145.674815	275347.088859	38.087616
2147.729832	275679.039671	38.092634
2149.719677	276019.155298	38.097652
2151.684948	276364.050635	38.102669
2153.724709	276719.273307	38.107687
2155.958521	277068.698582	38.112704
2157.722982	277420.459130	38.117722
2159.857574	277782.804932	38.122740
2161.877921	278137.649360	38.127757
2163.946871	278508.921971	38.132775
2166.176767	278873.945117	38.137792
2168.480864	279248.508036	38.142810
2170.348205	279620.345700	38.147828
2172.653606	279989.929057	38.152845
2174.383813	280377.716031	38.157863
2177.154953	280753.220365	38.162880
2179.687508	281137.069213	38.167898
2181.895028	281500.799176	38.172916
2184.635659	281867.137141	38.177933
2188.051042	282219.726341	38.182951
2190.352089	282573.279524	38.187968
2192.710351	282923.368566	38.192986
2194.724260	283283.800272	38.198004
2197.086819	283620.627680	38.203021
2198.912768	283980.199561	38.208039
2201.215777	284334.843515	38.213056
2203.250779	284687.294203	38.218074
2205.271783	285047.875810	38.223092
2207.614031	285393.901004	38.228109
2209.604514	285770.820980	38.233127
2211.740183	286117.919808	38.238144
2214.115609	286478.901142	38.243162
2216.027867	286843.181727	38.248180
2218.437306	287207.789546	38.253197
2220.109202	287591.769325	38.258215
2222.394320	287957.869397	38.263232
2224.649886	288334.414308	38.268250
2226.327445	288719.331724	38.273268
2228.959085	289089.693986	38.278285
2231.097135	289469.355239	38.283303
2233.320213	289854.718116	38.288320
2235.783519	290232.675585	38.293338
2238.162891	290606.530600	38.298356
2240.492405	290983.441302	38.303373
2242.187069	291352.170860	38.308391
2244.496447	291705.916522	38.313408
2246.946346	292058.242257	38.318426
2249.070925	292420.017967	38.323444
2250.846106	292759.519775	38.328461
2253.444705	293117.561298	38.333479
2255.770294	293472.089208	38.338496
2257.705825	293827.770689	38.343514
2259.857987	294190.580684	38.348532
2262.216212	294552.773142	38.353549
2264.191121	294925.897876	38.358567
2266.089692	295288.365139	38.363584
2268.243038	295667.124901	38.368602
2270.359773	296060.749933	38.373620
2273.241314	296439.926201	38.378637
2275.248377	296827.800801	38.383655
2277.570496	297218.876093	38.388672
2279.938210	297611.010202	38.393690
2281.963350	297996.694916	38.398708
2284.443583	298382.408254	38.403725
2286.663646	298784.469851	38.408743
2288.759878	299178.370823	38.413760
2291.250181	299575.942434	38.418778
2293.374837	299989.472381	38.423796
2296.390593	300389.498881	38.428813
2298.332491	300791.599721	38.433831
2300.893152	301193.626853	38.438848
2303.581173	301583.617986	38.443866
2305.723746	301990.357750	38.448884
2308.529886	302378.016624	38.453901
2310.889633	302779.385600	38.458919
2313.387904	303169.326498	38.463936
2315.514068	303556.759844	38.468954
2317.936166	303949.606405	38.473972
2320.461100	304340.047904	38.478989
2323.111806	304734.024464	38.484007
2325.354540	305122.222429	38.489024
2328.049535	305509.966586	38.494042
2330.585655	305901.925878	38.499060
2332.997971	306279.374621	38.504077
2335.555019	306657.307338	38.509095
2337.726418	307028.746819	38.514112
2340.419948	307400.966063	38.519130
2342.336787	307797.056387	38.524148
2344.864048	308173.465303	38.529165
2347.044651	308566.895158	38.534183
2349.200536	308949.634330	38.539200
2351.202711	309350.608268	38.544218
2353.389784	309748.808383	38.549236
2355.912311	310131.485640	38.554253
2357.802152	310527.545852	38.559271
2360.061322	310939.395386	38.564288
2362.646259	311337.907958	38.569306
2364.904965	311749.348226	38.574324
2366.859695	312144.351120	38.579341
2369.786261	312532.594816	38.584359
2371.945711	312919.942753	38.589376
2374.681273	313284.085030	38.594394
2376.674488	313659.214394	38.599412
2379.298062	314015.371302	38.604429
2381.428506	314379.300928	38.609447
2383.883970	314754.886474	38.614464
2386.544202	315114.589587	38.619482
2388.595386	315492.979525	38.624500
2390.957629	315883.535288	38.629517
2393.186128	316254.503372	38.634535
2395.558965	316641.041577	38.639552
2397.906035	317035.379505	38.644570
2399.921805	317422.631550	38.649588
2402.920763	317811.961220	38.654605
2406.046033	318199.770825	38.659623
2408.131997	318591.096018	38.664640
2410.921300	318963.945792	38.669658
2413.192547	319348.355748	38.674676
2415.366029	319730.646230	38.679693
2418.174656	320124.567908	38.684711
2420.364451	320514.217661	38.689728
2423.249093	320888.339712	38.694746
2425.947218	321283.975402	38.699764
2428.260949	321668.952853	38.704781
2430.573092	322066.423951	38.709799
2432.819145	322450.722965	38.714816
2435.554685	322834.460166	38.719834
2437.413255	323242.232416	38.724852
2439.652399	323640.952191	38.729869
2442.238116	324050.840154	38.734887
2444.559575	324454.647585	38.739904
2447.036576	324859.647386	38.744922
2449.282346	325270.522802	38.749940
2451.867313	325688.122968	38.754957
2453.924310	326114.515216	38.759975
2456.161659	326531.455006	38.764992
2458.759826	326951.205065	38.770010
2461.273972	327383.689031	38.775028
2463.567718	327812.497889	38.780045
2466.050123	328237.465283	38.785063
2468.327630	328678.486690	38.790080
2470.887357	329107.373131	38.795098
2473.247050	329555.588391	38.800116
2475.746662	330000.528363	38.805133
2478.293792	330433.700783	38.810151
2480.748744	330886.311443	38.815168
2483.404126	331320.426433	38.820186
2485.889430	331776.708808	38.825204
2488.427319	332211.675035	38.830221
2490.971357	332653.696911	38.835239
2493.183868	333098.663347	38.840256
2496.219571	333544.766174	38.845274
2498.876160	333990.723072	38.850292
2501.334558	334425.586613	38.855309
2504.082127	334847.299172	38.860327
2506.185638	335273.529395	38.865344
2509.238922	335655.246696	38.870362
2511.480038	336061.771360	38.875380
2513.705509	336464.487279	38.880397
2516.348389	336869.115161	38.885415
2518.784847	337283.853630	38.890432
2521.024115	337685.925120	38.895450
2523.518182	338106.286082	38.900468
2525.861359	338514.023567	38.905485
2528.536848	338928.561305	38.910503
2531.181645	339355.212497	38.915520
2534.104315	339772.143068	38.920538
2536.338838	340184.965126	38.925556
2538.690909	340619.093460	38.930573
2541.159779	341039.312013	38.935591
2543.613062	341471.310984	38.940608
2545.862751	341910.321277	38.945626
2548.431741	342355.853655	38.950644
2551.034999	342791.551738	38.955661
2553.411355	343241.982803	38.960679
2555.542605	343700.852974	38.965696
2558.383226	344145.795856	38.970714
2560.806644	344617.306905	38.975732
2563.141427	345077.098881	38.980749
2566.003180	345554.245256	38.985767
2568.498443	346011.186345	38.990784
2571.233632	346490.299873	38.995802
2573.642585	346955.904235	39.000820
2576.533443	347436.356045	39.005837
2579.395119	347887.131114	39.010855
2582.430079	348348.232867	39.015872
2585.641247	348811.486119	39.020890
2588.401063	349268.917372	39.025908
2590.981273	349716.371163	39.030925
2594.218150	350158.563942	39.035943
2596.871606	350606.227285	39.040960
2599.720101	351045.072662	39.045978
2602.301199	351489.033846	39.050996
2604.787735	351926.456980	39.056013
2607.722198	352358.880902	39.061031
2610.188181	352809.423921	39.066048
2612.857779	353246.324795	39.071066
2615.483717	353689.879569	39.076084
2617.710591	354151.694030	39.081101
2619.954067	354590.301019	39.086119
2622.744439	355035.848854	39.091136
2625.345195	355485.890279	39.096154
2627.554648	355949.290391	39.101172
2630.222822	356401.470536	39.106189
2632.881984	356851.084385	39.111207
2635.459016	357325.480340	39.116224
2638.307286	357779.193152	39.121242
2640.922707	358235.121502	39.126260
2643.418293	358693.907329	39.131277
2646.007065	359147.090170	39.136295
2648.379752	359588.348474	39.141312
2651.284518	360015.888910	39.146330
2653.738992	360441.923247	39.151348
2656.277449	360873.168854	39.156365
2658.589644	361297.213008	39.161383
2661.103755	361739.774163	39.166400
2663.396684	362179.345986	39.171418
2665.879330	362630.202897	39.176436
2668.417369	363100.740976	39.181453
2671.244803	363545.138812	39.186471
2674.020494	364019.715902	39.191488
2677.103044	364466.196232	39.196506
2679.418035	364928.020693	39.201524
2682.113712	365391.074437	39.206541
2685.441501	365843.440803	39.211559
2688.050855	366295.028169	39.216576
2691.478959	366758.180202	39.221594
2694.442071	367202.393701	39.226612
2696.841878	367662.983781	39.231629
2699.456513	368120.743608	39.236647
2702.255675	368583.316270	39.241664
2704.894210	369038.931082	39.246682
2707.584416	369514.884168	39.251700
2710.106810	369976.546880	39.256717
2713.102886	370439.905867	39.261735
2715.558931	370913.140008	39.266752
2717.841127	371398.779161	39.271770
2720.799034	371866.899024	39.276788
2723.478337	372355.509176	39.281805
2726.046279	372836.544541	39.286823
2728.732369	373325.091517	39.291840
2731.236276	373819.827224	39.296858
2734.141885	374326.240951	39.301876
2736.216991	374821.717562	39.306893
2739.381528	375315.188860	39.311911
2742.096544	375825.648315	39.316928
2744.352573	376342.288516	39.321946
2747.579429	376852.780766	39.326964
2750.366120	377371.074286	39.331981
2752.870661	377878.090497	39.336999
2755.859219	378400.879915	39.342016
2759.048980	378893.313608	39.347034
2761.892779	379404.594687	39.352052
2764.956069	379918.092162	39.357069
2768.229649	380405.698711	39.362087
2771.001436	380922.171805	39.367104
2773.888502	381421.064940	39.372122
2776.586392	381915.313837	39.377140
2779.623011	382415.768460	39.382157
2782.427798	382907.755177	39.387175
2785.663361	383397.764759	39.392192
2788.413984	383882.847521	39.397210
2791.173170	384374.517838	39.402228
2793.376346	384865.255054	39.407245
2796.331284	385350.666819	39.412263
2798.834277	385810.601004	39.417280
2801.134521	386282.609841	39.422298
2804.069979	386740.662979	39.427316
2806.752584	387207.577136	39.432333
2809.108382	387671.645535	39.437351
2811.794452	388157.975620	39.442368
2814.567455	388636.422767	39.447386
2817.422707	389111.578688	39.452404
2819.978594	389608.866435	39.457421
2822.711760	390097.698910	39.462439
2825.418226	390593.782331	39.467456
2828.192907	391101.564954	39.472474
2831.014016	391598.148626	39.477492
2833.532372	392107.504243	39.482509
2836.364454	392616.549123	39.487527
2839.453157	393121.995487	39.492544
2842.517046	393646.305901	39.497562
2845.482143	394157.690738	39.502580
2848.183149	394681.662338	39.507597
2851.181163	395194.902940	39.512615
2853.879026	395718.174341	39.517632
2856.524743	396247.658493	39.522650
2860.208387	396766.066369	39.527668
2863.129825	397286.437898	39.532685
2866.114756	397811.253969	39.537703
2869.137132	398335.371179	39.542720
2871.858342	398860.947644	39.547738
2875.214366	399379.974976	39.552756
2877.856215	399907.854532	39.557773
2880.878048	400427.577316	39.562791
2883.722821	400960.529235	39.567808
2886.504959	401493.583682	39.572826
2889.567087	402023.593294	39.577844
2892.349210	402558.759703	39.582861
2894.994667	403087.397854	39.587879
2898.020637	403634.803433	39.592896
2900.971954	404174.124229	39.597914
2904.080479	404703.523995	39.602932
2906.863452	405243.562893	39.607949
2910.017288	405780.593127	39.612967
2912.813116	406315.820213	39.617984
2915.421471	406859.863912	39.623002
2918.615088	407395.414912	39.628020
2921.621557	407955.650159	39.633037
2924.220907	408497.283507	39.638055
2927.179938	409042.221502	39.643072
2929.932255	409610.653734	39.648090
2932.969980	410159.792083	39.653108
2935.640675	410725.098578	39.658125
2938.143989	411281.930118	39.663143
2941.124610	411846.228557	39.668160
2944.124653	412429.623025	39.673178
2947.097929	412987.666105	39.678196
2950.465594	413546.219093	39.683213
2953.527850	414102.351483	39.688231
2956.487376	414634.413989	39.693248
2959.173643	415156.170375	39.698266
2962.081644	415662.753227	39.703284
2965.069610	416200.459032	39.708301
2967.780959	416721.600298	39.713319
2970.491004	417254.870339	39.718336
2973.300701	417796.350116	39.723354
2976.113428	418333.967508	39.728372
2978.609650	418890.882373	39.733389
2981.208466	419444.628044	39.738407
2984.198550	420019.458051	39.743424
2986.593253	420598.373775	39.748442
2989.755115	421168.490874	39.753460
2992.591166	421763.806803	39.758477
2995.294126	422355.203931	39.763495
2998.385711	422946.602871	39.768512
3001.071279	423557.003647	39.773530
3004.130985	424161.074056	39.778548
3007.078618	424777.182217	39.783565
3010.116393	425395.212740	39.788583
3013.236028	426018.915936	39.793600
3015.867498	426660.211480	39.798618
3019.179350	427278.509952	39.803636
3021.971686	427920.990984	39.808653
3024.683362	428566.255513	39.813671
3028.303335	429203.128530	39.818688
3031.247949	429863.724670	39.823706
3034.768943	430494.199184	39.828724
3037.949100	431141.681786	39.833741
3040.936029	431790.749082	39.838759
3044.318071	432428.948616	39.843776
3047.128191	433085.026694	39.848794
3050.802546	433734.265478	39.853812
3053.795632	434372.604811	39.858829
3057.101706	435021.362591	39.863847
3060.737049	435649.616008	39.868864
3063.748739	436296.640351	39.873882
3067.247781	436922.148766	39.878900
3070.289063	437565.489365	39.883917
3073.397427	438205.485777	39.888935
3076.407738	438834.315188	39.893952
3079.159690	439468.283951	39.898970
3082.857450	440099.251101	39.903988
3086.215632	440730.053206	39.909005
3089.081200	441371.600809	39.914023
3092.348386	441985.067922	39.919040
3094.977780	442642.264954	39.924058
3098.074194	443276.789115	39.929076
3101.079587	443916.525735	39.934093
3104.645560	444546.739864	39.939111
3107.434085	445198.677780	39.944128
3110.500126	445835.012092	39.949146
3113.725644	446474.088389	39.954164
3116.726501	447113.739775	39.959181
3119.454484	447752.708245	39.964199
3122.651447	448353.569897	39.969216
3125.418213	448954.129815	39.974234
3128.322557	449575.506620	39.979252
3131.301883	450187.895972	39.984269
3134.107215	450803.991450	39.989287
3137.301972	451415.706754	39.994304
3139.926658	452059.532950	39.999322
3143.379691	452686.913573	40.004340
3146.355356	453320.526670	40.009357
3148.901513	453968.410625	40.014375
3151.960667	454591.600498	40.019392
3154.983012	455266.901362	40.024410
3157.986509	455925.536596	40.029428
3161.138935	456591.010642	40.034445
3163.839707	457275.915930	40.039463
3167.187082	457950.426391	40.044480
3170.001906	458635.929366	40.049498
3173.226781	459334.450245	40.054516
3176.615238	460025.839944	40.059533
3179.819663	460732.313215	40.064551
3182.918102	461441.411008	40.069568
3186.150850	462147.429070	40.074586
3189.824599	462849.914409	40.079604
3193.063767	463555.935922	40.084621
3196.140053	464295.344989	40.089639
3199.736938	465001.363396	40.094656
3202.919964	465731.752791	40.099674
3206.516542	466427.203197	40.104692
3210.630936	467109.955214	40.109709
3213.946290	467816.682821	40.114727
3217.761698	468514.962922	40.119744
3220.976846	469211.898593	40.124762
3224.224476	469905.114176	40.129780
3227.770470	470600.029273	40.134797
3230.665030	471292.293416	40.139815
3234.086335	471991.176084	40.144832
3236.768011	472689.292322	40.149850
3240.000317	473378.651643	40.154868
3243.619482	474094.470220	40.159885
3246.233124	474795.811344	40.164903
3249.980545	475489.618209	40.169920
3253.045550	476210.555621	40.174938
3255.854169	476923.065416	40.179956
3259.530180	477631.621353	40.184973
3262.945440	478333.975804	40.189991
3266.613817	479028.582216	40.195008
3270.428402	479733.755625	40.200026
3273.573396	480422.532498	40.205044
3277.345360	481108.153570	40.210061
3280.563415	481801.217046	40.215079
3283.853019	482492.526287	40.220096
3287.108603	483179.419658	40.225114
3290.337834	483874.226773	40.230132
3293.876728	484545.007380	40.235149
3297.177905	485227.525392	40.240167
3300.496134	485869.845648	40.245184
3303.174167	486523.462681	40.250202
3306.275453	487158.093696	40.255220
3309.699886	487812.609479	40.260237
3312.243209	488468.909199	40.265255
3314.978313	489122.831838	40.270272
3318.073681	489792.739808	40.275290
3321.342776	490468.759472	40.280308
3324.267306	491143.041146	40.285325
3327.115463	491854.336790	40.290343
3330.430042	492541.892133	40.295360
3333.615799	493257.677130	40.300378
3336.758711	493967.885317	40.305396
3340.260230	494687.251906	40.310413
3342.930765	495406.570137	40.315431
3345.858173	496161.170512	40.320448
3348.966918	496901.571119	40.325466
3351.794010	497672.183441	40.330484
3355.125072	498441.117903	40.335501
3358.501084	499223.443567	40.340519
3362.145602	500005.238277	40.345536
3365.205975	500785.526023	40.350554
3368.488800	501589.018623	40.355572
3372.372486	502383.545191	40.360589
3375.753764	503175.036123	40.365607
3379.397469	503977.151683	40.370624
3382.959938	504776.366269	40.375642
3386.250964	505581.745207	40.380660
3389.939164	506382.532127	40.385677
3393.036810	507187.564530	40.390695
3396.829484	507997.546895	40.395712
3400.253653	508796.396635	40.400730
3403.542300	509636.711297	40.405748
3407.698053	510432.694698	40.410765
3410.968535	511256.684316	40.415783
3414.342228	512068.911979	40.420800
3417.703399	512875.653744	40.425818
3421.381409	513693.355654	40.430836
3425.015473	514499.572982	40.435853
3428.121375	515321.271535	40.440871
3431.927081	516133.386139	40.445888
3435.445031	516954.485143	40.450906
3438.516305	517776.068080	40.455924
3442.597748	518589.279898	40.460941
3445.744225	519411.425249	40.465959
3449.584459	520226.662039	40.470976
3453.367099	521034.050898	40.475994
3456.864715	521852.841136	40.481012
3460.390133	522653.332425	40.486029
3463.700329	523465.767971	40.491047
3467.581048	524264.711568	40.496064
3470.817431	525066.843132	40.501082
3474.330791	525880.233846	40.506100
3477.853753	526669.132358	40.511117
3481.747963	527463.921562	40.516122
3484.717368	528204.464515	40.521127
3488.182487	528898.101192	40.526132
3491.393092	529527.219939	40.531136
3494.445455	530096.866093	40.536141
3496.624165	530627.066876	40.541146
3499.429660	531073.480158	40.546151
3502.063722	531481.307129	40.551156
3503.829986	531824.893941	40.556160
3505.828040	532121.450773	40.561165
3507.794348	532360.766059	40.566170
3509.603742	532558.422689	40.571175
3511.341907	532711.175397	40.576180
3512.356239	532831.455554	40.581184
3513.812622	532899.124317	40.586189
3514.646658	532952.695102	40.591194
3515.602796	532943.753603	40.596199
3516.329811	532919.591327	40.601204
3517.073427	532891.485839	40.606208
3518.097201	532819.333036	40.611213
3518.794889	532721.567056	40.616218
3519.434394	532606.885186	40.621223
3519.913314	532470.604757	40.626228
3520.391197	532310.578074	40.631232
3520.776627	532135.862358	40.636237
3521.027362	531956.972570	40.641242
3521.653784	531745.332608	40.646247
3521.976171	531532.575771	40.651252
3522.147279	531318.930498	40.656256
3522.245409	531075.332077	40.661261
3521.989103	530828.804813	40.666266
3522.487458	530585.539746	40.671271
3522.300385	530329.696661	40.676276
3522.048797	530069.059348	40.681280
3522.587718	529806.423186	40.686285
3522.265082	529552.155305	40.691290
3522.153186	529288.754345	40.696295
3521.976540	529007.622347	40.701300
3521.815014	528743.462147	40.706304
3521.522364	528468.453418	40.711309
3521.179108	528196.378940	40.716314
3521.552337	527933.485164	40.721319
3520.980256	527673.263260	40.726324
3520.735527	527389.586472	40.731328
3520.698302	527128.260366	40.736333
3520.404680	526870.558777	40.741338
3520.086134	526611.694538	40.746343
3520.237566	526346.838542	40.751348
3519.672097	526091.492211	40.756352
3519.715220	525832.810899	40.761357
3519.499603	525572.447825	40.766362
3519.472205	525313.011113	40.771367
3519.165732	525054.220849	40.776372
3518.748763	524811.567974	40.781376
3518.897335	524562.756479	40.786381
3518.398435	524335.374408	40.791386
3518.037776	524087.798634	40.796391
3518.129019	523848.943128	40.801396
3517.473437	523628.248276	40.806400
3517.360290	523391.136979	40.811405
3517.384171	523157.185258	40.816410
3517.040793	522916.665928	40.821415
3516.875531	522718.326097	40.826420
3516.368433	522492.941479	40.831424
3516.594815	522275.930833	40.836429
3516.580820	522070.886098	40.841434
3516.017334	521866.380612	40.846439
3515.902068	521651.791710	40.851444
3515.532584	521450.839791	40.856448
3515.359418	521245.809818	40.861453
3515.305874	521046.572476	40.866458
3514.998058	520856.625018	40.871463
3514.982059	520663.797948	40.876468
3514.616480	520478.456062	40.881472
3514.693439	520281.817855	40.886477
3514.195021	520110.396748	40.891482
3513.468497	519921.920301	40.896487
3513.591578	519745.593867	40.901492
3513.362514	519590.456114	40.906496
3513.479545	519410.638264	40.911501
3513.149989	519236.552090	40.916506
3513.196424	519081.416557	40.921511
3512.821041	518925.183254	40.926516
3512.813901	518778.750348	40.931520
3512.910593	518626.585894	40.936525
3512.556075	518448.551271	40.941530
3512.339313	518310.541206	40.946535
3512.126073	518158.016886	40.951540
3511.882527	518012.170771	40.956544
3512.055281	517857.104900	40.961549
3511.704053	517722.195778	40.966554
3511.447912	517587.523370	40.971559
3511.503455	517449.918202	40.976564
3511.156709	517304.739555	40.981568
3510.819820	517182.921137	40.986573
3510.776013	517077.490659	40.991578
3510.849918	516931.686002	40.996583
3511.041094	516798.706450	41.001588
3510.694041	516678.049057	41.006592
3510.659363	516565.432820	41.011597
3510.251889	516439.169835	41.016602
3510.238591	516322.957993	41.021607
3510.625309	516196.871089	41.026612
3509.983226	516111.201671	41.031616
3510.303019	515985.882337	41.036621
3509.920017	515863.050081	41.041626
3509.882339	515775.867365	41.046631
3509.558257	515657.120745	41.051636
3509.487285	515549.813652	41.056640
3509.571354	515451.584799	41.061645
3509.294886	515336.014572	41.066650
3509.517421	515228.305005	41.071655
3509.390996	515130.967316	41.076660
3508.926765	515054.317391	41.081664
3509.140673	514939.425563	41.086669
3509.071442	514854.164924	41.091674
3509.001211	514760.609433	41.096679
3509.212696	514667.110051	41.101684
3508.959815	514579.095304	41.106688
3508.945248	514473.036828	41.111693
3508.508117	514381.914356	41.116698
3508.630598	514295.103242	41.121703
3508.680875	514209.466394	41.126708
3508.124434	514130.449636	41.131712
3508.351302	514036.742001	41.136717
3508.321243	513950.357847	41.141722
3508.103458	513872.146198	41.146727
3508.190962	513790.547683	41.151732
3508.070202	513718.490699	41.156736
3508.439756	513630.423193	41.161741
3508.152855	513560.414994	41.166746
3508.092533	513480.962715	41.171751
3508.069033	513390.022402	41.176756
3508.029088	513320.834052	41.181760
3508.064211	513234.739414	41.186765
3508.071420	513161.192966	41.191770
3507.966694	513084.780730	41.196775
3507.645325	513005.923871	41.201780
3507.546228	512937.754939	41.206784
3507.747027	512863.923691	41.211789
3507.551182	512803.103952	41.216794
3507.365344	512724.274941	41.221799
3507.572109	512652.161642	41.226804
3507.043122	512604.343087	41.231808
3506.908620	512526.213204	41.236813
3507.143937	512457.989488	41.241818
3506.878305	512397.533405	41.246823
3507.351329	512347.937084	41.251828
3507.039104	512280.861452	41.256832
3507.085701	512217.573254	41.261837
3506.933170	512166.760075	41.266842
3507.062383	512106.139382	41.271847
3507.073084	512040.276378	41.276852
3506.893266	511989.669320	41.281856
3506.932010	511926.887129	41.286861
3506.787218	511865.297176	41.291866
3506.644018	511809.524086	41.296871
3506.545457	511749.089872	41.301876
3506.884111	511694.858995	41.306880
3506.581913	511636.328241	41.311885
3506.490675	511583.783704	41.316890
3506.548921	511549.679395	41.321895
3506.390459	511482.222200	41.326900
3505.992246	511435.947862	41.331904
3506.103211	511387.468280	41.336909
3506.198067	511351.688424	41.341914
3506.358710	511299.457310	41.346919
3506.281077	511250.349512	41.351924
3506.113838	511216.128409	41.356928
3506.319617	511168.290854	41.361933
3505.708457	511128.221000	41.366938
3505.911545	511080.029510	41.371943
3506.427806	511035.481302	41.376948
3505.967332	510988.608532	41.381952
3506.208840	510946.127033	41.386957
3506.321058	510893.851741	41.391962
3506.172392	510859.019926	41.396967
3506.054237	510806.123125	41.401972
3505.995036	510769.911099	41.406976
3506.099500	510717.990614	41.411981
3506.035587	510681.323845	41.416986
3505.978409	510647.741862	41.421991
3506.215626	510611.128529	41.426996
3506.182511	510562.922320	41.432000
3506.244917	510525.678771	41.437005
3506.059596	510471.071509	41.442010
3505.917870	510427.941035	41.447015
3506.042099	510385.628446	41.452020
3506.296534	510329.888848	41.457024
3505.881931	510296.109712	41.462029
3505.919319	510253.102259	41.467034
3506.006493	510206.494919	41.472039
3506.343742	510150.589878	41.477044
3506.148283	510119.254690	41.482048
3505.933191	510073.048892	41.487053
3505.855519	510021.155076	41.492058
3505.837217	509984.681968	41.497063
3505.985814	509951.015504	41.502068
3505.740342	509916.348839	41.507072
3505.974421	509870.880965	41.512077
3505.888186	509836.391337	41.517082
3505.618289	509794.746673	41.522087
3505.825917	509749.485024	41.527092
3505.331652	509712.681825	41.532096
3505.763522	509676.693424	41.537101
3505.873302	509642.981898	41.542106
3505.909731	509600.478878	41.547111
3506.092192	509567.716967	41.552116
3506.052985	509528.109476	41.557120
3505.757665	509471.189162	41.562125
3505.591643	509440.505782	41.567130
3505.528509	509404.240895	41.572135
3505.635310	509358.589408	41.577140
3505.521355	509324.963210	41.582144
3505.404842	509288.251178	41.587149
3505.400764	509276.109533	41.592154
3505.121077	509248.985287	41.597159
3505.428448	509210.182371	41.602164
3505.430313	509185.239629	41.607168
3505.625414	509132.692896	41.612173
3505.568534	509120.812454	41.617178
3505.479430	509078.327981	41.622183
3505.477753	509035.020085	41.627188
3505.285400	509008.792345	41.632192
3505.233322	508976.977064	41.637197
3505.180260	508946.021979	41.642202
3505.245551	508929.720416	41.647207
3505.440090	508890.681642	41.652212
3505.240638	508869.514227	41.657216
3504.872894	508829.299323	41.662221
3505.251933	508807.534462	41.667226
3505.316766	508777.369951	41.672231
3505.479551	508744.356609	41.677236
3505.208233	508727.652703	41.682240
3505.416357	508687.650023	41.687245
3505.322213	508655.334848	41.692250
3505.429731	508622.835956	41.697255
3505.336373	508591.228866	41.702260
3505.095630	508566.171785	41.707264
3505.595847	508541.807086	41.712269
3505.483324	508513.289189	41.717274
3505.392083	508486.386933	41.722279
3505.313080	508440.307018	41.727284
3505.446681	508424.297754	41.732288
3505.209961	508388.715902	41.737293
3505.247450	508359.162129	41.742298
3505.390962	508329.085590	41.747303
3505.652889	508283.507928	41.752308
3505.232785	508260.603779	41.757312
3505.210683	508222.609651	41.762317
3505.530146	508204.091598	41.767322
3505.260247	508165.934124	41.772327
3505.459156	508126.285773	41.777332
3504.982780	508095.294868	41.782336
3505.209839	508062.674836	41.787341
3505.136436	508037.539941	41.792346
3505.192525	508012.080965	41.797351
3505.365345	507979.368154	41.802356
3505.261948	507953.478925	41.807360
3505.373275	507917.739901	41.812365
3505.584977	507882.440313	41.817370
3505.370371	507862.083609	41.822375
3505.415956	507830.706153	41.827380
3505.591152	507805.784619	41.832384
3505.177904	507770.279987	41.837389
3504.923121	507732.321555	41.842394
3505.009935	507717.583971	41.847399
3505.521919	507683.299069	41.852404
3505.510025	507656.737164	41.857408
3505.249496	507623.687386	41.862413
3505.197774	507597.030488	41.867418
3504.857401	507568.192854	41.872423
3505.557018	507536.306714	41.877428
3505.365406	507517.818102	41.882432
3505.442744	507477.883890	41.887437
3505.288392	507452.305554	41.892442
3505.207660	507420.238939	41.897447
3505.402649	507377.351189	41.902452
3505.251877	507360.272715	41.907456
3505.034846	507330.302020	41.912461
3505.267205	507304.206959	41.917466
3504.855366	507277.960675	41.922471
3505.120522	507242.044148	41.927476
3505.128847	507215.225375	41.932480
3505.235426	507195.221917	41.937485
3505.080191	507151.680571	41.942490
3504.810985	507144.436858	41.947495
3505.315712	507100.892280	41.952500
3505.072436	507086.003930	41.957504
3504.974722	507059.100476	41.962509
3505.207649	507032.144724	41.967514
3504.790966	507008.175779	41.972519
3505.028355	506983.951630	41.977524
3504.743268	506956.470432	41.982528
3504.629638	506929.316292	41.987533
3504.801670	506910.769560	41.992538
3504.698520	506892.418099	41.997543
3505.189192	506864.156351	42.002548
3504.771736	506849.902527	42.007552
3504.623392	506822.500706	42.012557
3505.085202	506804.110463	42.017562
3504.823737	506786.087512	42.022567
3504.750787	506758.370072	42.027572
3504.780058	506733.672462	42.032576
3505.068290	506718.800996	42.037581
3505.095737	506688.638751	42.042586
3504.417912	506666.380426	42.047591
3504.968637	506638.260622	42.052596
3505.097050	506623.464934	42.057600
3505.055830	506592.604964	42.062605
3505.068917	506565.531430	42.067610
3504.974655	506542.573505	42.072615
3505.007868	506510.639004	42.077620
3505.054802	506487.658692	42.082624
3505.126331	506461.587784	42.087629
3505.166418	506446.451695	42.092634
3505.053020	506413.882370	42.097639
3505.555003	506380.507306	42.102644
3504.934621	506350.952877	42.107648
3504.798612	506331.442179	42.112653
3505.096472	506304.829250	42.117658
3504.893316	506284.215873	42.122663
3505.201242	506254.059150	42.127668
3504.995571	506234.407547	42.132672
3504.990510	506199.391806	42.137677
3504.952053	506185.229342	42.142682
3504.788825	506165.823965	42.147687
3505.047314	506130.513422	42.152692
3505.134732	506118.658714	42.157696
3504.752124	506074.391568	42.162701
3504.975831	506058.871906	42.167706
3504.886922	506028.119677	42.172711
3504.960208	506005.083960	42.177716
3504.736228	505972.986710	42.182720
3504.900339	505952.517307	42.187725
3505.036936	505927.852194	42.192730
3504.855879	505909.512008	42.197735
3504.867660	505869.230241	42.202740
3504.937630	505852.165999	42.207744
3504.678125	505839.404473	42.212749
3505.013639	505809.849858	42.217754
3504.876310	505790.439969	42.222759
3505.013277	505770.278262	42.227764
3504.732429	505743.654732	42.232768
3504.386691	505719.470381	42.237773
3504.805101	505692.786863	42.242778
3504.754844	505692.390014	42.247783
3504.600101	505662.659615	42.252788
3504.599300	505646.820844	42.257792
3504.864165	505616.720429	42.262797
3504.979966	505610.275488	42.267802
3505.009373	505590.434195	42.272807
3504.998726	505564.830368	42.277812
3504.638752	505540.698623	42.282816
3505.021554	505512.907172	42.287821
3504.980194	505484.474254	42.292826
3504.630091	505473.548526	42.297831
3504.661921	505451.935547	42.302836
3504.813577	505437.995452	42.307840
3504.782541	505400.249581	42.312845
3505.002939	505384.679240	42.317850
3504.727173	505363.013556	42.322855
3504.750089	505342.565754	42.327860
3504.825749	505324.791634	42.332864
3504.783947	505295.447597	42.337869
3504.882913	505267.042753	42.342874
3504.562947	505256.972406	42.347879
3505.006737	505225.375501	42.352884
3504.785367	505199.450208	42.357888
3504.659286	505180.088468	42.362893
3504.688960	505157.311550	42.367898
3504.614185	505137.739234	42.372903
3504.721058	505118.239398	42.377908
3504.445970	505097.129934	42.382912
3504.573637	505078.082214	42.387917
3504.858345	505074.241856	42.392922
3504.771324	505061.199473	42.397927
3504.298630	505038.248770	42.402932
3504.476892	505012.158829	42.407936
3504.448180	505002.851992	42.412941
3504.399019	504979.277615	42.417946
3504.311585	504955.152592	42.422951
3504.534593	504950.815903	42.427956
3504.365211	504935.357370	42.432960
3504.154556	504916.615973	42.437965
3504.432067	504904.376158	42.442970
3504.325204	504893.867075	42.447975
3504.512907	504866.763309	42.452980
3504.499017	504862.211009	42.457984
3504.999129	504841.788415	42.462989
3505.038224	504833.533497	42.467994
3504.607225	504800.252265	42.472999
3504.978156	504776.206373	42.478004
3504.975165	504759.253809	42.483008
3504.600216	504746.104877	42.488013
3505.369441	504693.858825	42.493018
3504.987869	504690.427325	42.498023
3504.789674	504655.337799	42.503028
3504.798243	504628.464402	42.508032
3504.740751	504596.945590	42.513037
3504.872200	504592.420857	42.518042
3504.811942	504561.610912	42.523047
3504.746104	504531.662112	42.528052
3504.863657	504520.661876	42.533056
3504.513572	504505.282129	42.538061
3504.550571	504475.519408	42.543066
3504.525121	504477.092285	42.548071
3504.455471	504440.261374	42.553076
3504.595632	504431.079366	42.558080
3504.599393	504416.554546	42.563085
3504.866950	504389.336208	42.568090
3504.730571	504380.197879	42.573095
3504.750522	504360.761545	42.578100
3504.828341	504350.475985	42.583104
3504.565192	504326.782728	42.588109
3505.001387	504294.982919	42.593114
3504.614090	504278.394273	42.598119
3504.735089	504253.628052	42.603124
3504.687040	504227.420889	42.608128
3504.586693	504210.837436	42.613133
3504.636426	504183.298950	42.618138
3504.927230	504170.854093	42.623143
3504.739417	504154.841097	42.628148
3504.803455	504129.678840	42.633152
3504.551354	504115.194210	42.638157
3504.761072	504091.122251	42.643162
3504.611517	504077.582938	42.648167
3504.537733	504043.535298	42.653172
3504.632068	504030.058618	42.658176
3504.930656	504010.881511	42.663181
3504.567037	503995.756498	42.668186
3504.635033	503963.963675	42.673191
3504.979320	503940.730588	42.678196
3504.724126	503918.908039	42.683200
3504.185451	503895.308353	42.688205
3504.718438	503880.446406	42.693210
3504.600591	503874.240191	42.698215
3504.354246	503857.679478	42.703220
3504.513986	503828.959049	42.708224
3504.411827	503814.804735	42.713229
3504.318058	503806.924596	42.718234
3504.348560	503783.842111	42.723239
3504.155519	503764.995481	42.728244
3504.197581	503762.053543	42.733248
3504.362929	503747.300197	42.738253
3504.523154	503722.273983	42.743258
3504.545809	503723.738106	42.748263
3504.798423	503708.717890	42.753268
3504.479057	503685.083260	42.758272
3504.535571	503674.800672	42.763277
3504.320439	503653.983650	42.768282
3504.169234	503653.703927	42.773287
3504.474646	503632.096078	42.778292
3504.735068	503606.193503	42.783296
3504.676906	503595.625336	42.788301
3505.005487	503574.671680	42.793306
3504.550570	503562.445470	42.798311
3504.466486	503528.499681	42.803316
3504.693943	503515.204007	42.808321
3504.840510	503497.265003	42.813325
3505.169231	503467.555692	42.818330
3504.669667	503455.893173	42.823335
3504.747663	503420.656311	42.828340
3504.889508	503398.163046	42.833345
3504.630233	503387.272268	42.838349
3504.704285	503351.681620	42.843354
3504.538081	503341.535258	42.848359
3504.383409	503307.903862	42.853364
3504.505890	503291.334935	42.858369
3504.509337	503288.044748	42.863373
3504.626008	503257.811882	42.868378
3504.359956	503241.051261	42.873383
3504.422178	503239.523146	42.878388
3504.570924	503214.801691	42.883393
3504.420267	503201.666762	42.888397
3504.657826	503189.836958	42.893402
3504.510667	503164.757312	42.898407
3504.777516	503149.683760	42.903412
3504.567541	503132.762341	42.908417
3504.705719	503112.344338	42.913421
3504.963276	503087.301841	42.918426
3504.508324	503066.268971	42.923431
3504.455585	503054.130678	42.928436
3504.763662	503030.699673	42.933441
3504.565894	503018.381832	42.938445
3504.614368	502995.599143	42.943450
3504.597575	502972.978574	42.948455
3504.667631	502958.948189	42.953460
3504.653088	502943.362209	42.958465
3504.389042	502927.360144	42.963469
3504.569477	502903.038136	42.968474
3504.357223	502895.581207	42.973479
3504.423972	502884.031252	42.978484
3504.688404	502862.175881	42.983489
3504.513729	502851.575070	42.988493
3504.367531	502822.192791	42.993498
3504.174967	502805.470753	42.998503
3504.764003	502787.005592	43.003508
3504.806411	502760.123996	43.008513
3504.347614	502758.526348	43.013517
3504.637410	502729.884800	43.018522
3504.190777	502726.311357	43.023527
3504.391031	502711.197345	43.028532
3504.559133	502682.777403	43.033537
3504.662790	502662.769234	43.038541
3504.781848	502655.816576	43.043546
3504.195179	502631.210533	43.048551
3504.506633	502616.584989	43.053556
3504.410565	502599.847505	43.058561
3504.225715	502588.843246	43.063565
3504.524679	502575.738016	43.068570
3504.567203	502545.515650	43.073575
3504.373580	502535.778059	43.078580
3504.582765	502520.105734	43.083585
3504.239533	502494.347547	43.088589
3504.504479	502489.750565	43.093594
3504.283684	502466.756688	43.098599
3504.470477	502441.977527	43.103604
3504.547085	502435.740072	43.108609
3504.544933	502426.377062	43.113613
3504.988579	502395.939208	43.118618
3504.610909	502371.097319	43.123623
3504.569064	502357.640886	43.128628
3504.440095	502336.960531	43.133633
3504.203680	502323.079304	43.138637
3504.607803	502309.805419	43.143642
3504.287223	502294.975820	43.148647
3504.621758	502266.579520	43.153652
3504.863988	502262.542817	43.158657
3504.423844	502241.860917	43.163661
3504.313147	502221.025698	43.168666
3504.406966	502221.618269	43.173671
3504.362070	502201.076308	43.178676
3504.456979	502174.387980	43.183681
3504.569345	502173.459212	43.188685
3504.627325	502139.437688	43.193690
3504.384663	502138.818098	43.198695
3504.594013	502112.769568	43.203700
3504.433623	502092.549418	43.208705
3504.137175	502094.317178	43.213709
3504.568248	502068.689066	43.218714
3504.424208	502049.326719	43.223719
3504.491224	502042.432660	43.228724
3504.793506	502032.211504	43.233729
3504.575216	502000.359166	43.238733
3504.385794	501975.082056	43.243738
3504.086229	501973.661625	43.248743
3504.200279	501954.359614	43.253748
3504.339119	501942.747037	43.258753
3504.339014	501930.599655	43.263757
3504.702632	501909.081735	43.268762
3504.641212	501892.692409	43.273767
3503.941007	501866.078666	43.278772
3504.361029	501860.039806	43.283777
3504.081254	501844.140475	43.288781
3504.307699	501824.466257	43.293786
3504.141082	501829.503474	43.298791
3504.091491	501811.644379	43.303796
3504.383796	501801.981428	43.308801
3503.813735	501788.608046	43.313805
3504.054666	501774.195414	43.318810
3503.980742	501773.903445	43.323815
3504.081512	501775.355384	43.328820
3504.347079	501744.185337	43.333825
3504.201814	501737.122250	43.338829
3504.365150	501727.631486	43.343834
3504.188488	501716.878465	43.348839
3504.528062	501696.983766	43.353844
3504.499860	501683.423436	43.358849
3504.301383	501668.067864	43.363853
3504.502789	501648.043102	43.368858
3504.298616	501639.420217	43.373863
3504.337477	501627.722006	43.378868
3504.523761	501608.458817	43.383873
3504.028456	501600.793000	43.388877
3504.399960	501573.655132	43.393882
3504.117639	501570.156713	43.398887
3504.204096	501560.070627	43.403892
3504.527588	501547.770610	43.408897
3504.300264	501536.569947	43.413901
3504.428859	501513.266536	43.418906
3504.097230	501509.168512	43.423911
3504.290449	501492.687956	43.428916
3504.148048	501477.171510	43.433921
3504.280505	501467.634873	43.438925
3504.733943	501446.405892	43.443930
3504.383147	501435.275295	43.448935
3504.298360	501423.596492	43.453940
3504.410305	501398.625242	43.458945
3504.139051	501378.674879	43.463949
3504.085397	501385.010382	43.468954
3504.062827	501378.737615	43.473959
3504.344902	501345.337160	43.478964
3504.621660	501339.928160	43.483969
3504.564637	501333.964518	43.488973
3504.657999	501296.645747	43.493978
3504.373890	501291.426607	43.498983
3504.623861	501272.811000	43.503988
3504.773737	501256.185228	43.508993
3504.615220	501238.190923	43.513997
3504.465674	501209.768211	43.519002
3504.620346	501199.164975	43.524007
3504.712916	501173.487842	43.529012
3504.436852	501164.623006	43.534017
3504.305713	501144.700852	43.539021
3504.483106	501111.063420	43.544026
3504.406084	501120.844643	43.549031
3504.233406	501096.778436	43.554036
3504.250386	501085.640111	43.559041
3504.108989	501069.870067	43.564045
3504.257285	501051.523382	43.569050
3504.037455	501036.879274	43.574055
3504.293326	501028.942638	43.579060
3504.453629	501016.769280	43.584065
3504.374166	501017.591746	43.589069
3504.474991	500997.126598	43.594074
3504.204558	500985.426230	43.599079
3504.618938	500960.406568	43.604084
3504.629735	500943.448165	43.609089
3504.205137	500944.780736	43.614093
3504.325376	500907.558136	43.619098
3504.307628	500903.157277	43.624103
3504.390667	500889.072588	43.629108
3504.622216	500870.206387	43.634113
3504.283877	500852.543816	43.639117
3504.675550	500834.715236	43.644122
3504.253957	500815.041088	43.649127
3504.190333	500805.788175	43.654132
3504.496050	500816.622660	43.659137
3504.249767	500781.937982	43.664141
3504.151069	500756.847272	43.669146
3504.370958	500758.179233	43.674151
3504.608087	500735.920625	43.679156
3504.672865	500728.621469	43.684161
3504.217012	500718.772470	43.689165
3504.413806	500704.467185	43.694170
3504.263887	500683.889453	43.699175
3504.133694	500669.180258	43.704180
3504.421660	500646.154234	43.709185
3504.450980	500633.090193	43.714189
3504.166848	500628.225187	43.719194
3504.193360	500610.555331	43.724199
3503.987482	500584.266483	43.729204
3504.098919	500577.466074	43.734209
3504.041203	500577.930795	43.739213
3504.169607	500559.029949	43.744218
3504.157790	500550.072425	43.749223
3504.395621	500526.750461	43.754228
3504.370604	500523.869207	43.759233
3504.546312	500508.605350	43.764237
3504.105406	500494.147592	43.769242
3504.345953	500483.479741	43.774247
3504.384027	500454.621225	43.779252
3504.464517	500435.221635	43.784257
3504.346875	500440.099647	43.789261
3504.702337	500408.153780	43.794266
3504.438079	500399.438552	43.799271
3504.414623	500376.157687	43.804276
3504.670776	500358.299432	43.809281
3504.363795	500361.790064	43.814285
3504.718220	500326.351518	43.819290
3504.368094	500309.145841	43.824295
3504.443990	500294.808718	43.829300
3504.444570	500278.458726	43.834305
3504.649120	500277.717768	43.839309
3504.694888	500250.173800	43.844314
3504.626843	500225.786167	43.849319
3504.562367	500210.863732	43.854324
3504.619348	500189.746538	43.859329
3504.618801	500175.421401	43.864333
3504.423433	500156.621919	43.869338
3504.264560	500144.549032	43.874343
3503.916706	500121.369725	43.879348
3504.402559	500113.041999	43.884353
3504.174395	500112.926238	43.889357
3504.310569	500104.400676	43.894362
3504.290381	500092.305835	43.899367
3504.074862	500064.802877	43.904372
3504.073212	500047.086296	43.909377
3504.257042	500052.422964	43.914381
3504.183435	500040.893347	43.919386
3504.248579	500026.709568	43.924391
3504.288692	500006.151640	43.929396
3504.183547	499995.892473	43.934401
3504.029813	499989.639948	43.939405
3504.294662	499963.984469	43.944410
3504.147376	499954.288757	43.949415
3503.973600	499957.201595	43.954420
3504.649100	499947.578322	43.959425
3504.447268	499935.410843	43.964429
3504.309580	499911.489368	43.969434
3504.456206	499899.469272	43.974439
3504.254415	499879.961834	43.979444
3504.543921	499873.588596	43.984449
3504.361127	499851.243394	43.989453
3504.562140	499824.534780	43.994458
3504.241198	499817.853038	43.999463
3503.816243	499804.860188	44.004468
3504.069470	499781.939785	44.009473
3504.163556	499778.330901	44.014477
3504.327517	499762.511441	44.019482
3504.370190	499779.209484	44.024487
3504.470739	499747.454589	44.029492
3504.672029	499737.096223	44.034497
3504.106575	499720.227733	44.039501
3504.306828	499698.783594	44.044506
3504.133167	499685.700320	44.049511
3504.380490	499670.778777	44.054516
3504.522895	499640.788804	44.059521
3504.450250	499647.735373	44.064525
3504.540967	499620.436438	44.069530
3504.268974	499610.152799	44.074535
3504.175984	499595.082494	44.079540
3504.509842	499576.249382	44.084545
3504.316782	499555.221579	44.089549
3504.399781	499552.272476	44.094554
3504.232811	499520.508839	44.099559
3504.254854	499506.128975	44.104564
3504.187831	499492.218767	44.109569
3504.329010	499492.247112	44.114573
3504.426127	499476.134237	44.119578
3504.183927	499464.377788	44.124583
3504.111072	499453.606994	44.129588
3504.374961	499434.784792	44.134593
3503.977352	499436.366311	44.139597
3503.967021	499411.867205	44.144602
3504.338927	499419.553547	44.149607
3504.140070	499409.207612	44.154612
3504.188346	499386.724068	44.159617
3504.347437	499382.396130	44.164621
3504.127478	499384.405170	44.169626
3504.177691	499355.188614	44.174631
3504.035394	499344.580594	44.179636
3504.312216	499336.538656	44.184641
3504.091546	499329.182801	44.189645
3504.243317	499305.569122	44.194650
3504.599089	499289.921418	44.199655
3504.085194	499294.609258	44.204660
3504.380320	499271.175364	44.209665
3504.259643	499249.325813	44.214669
3504.414424	499242.669913	44.219674
3504.428297	499232.442121	44.224679
3504.255573	499226.799793	44.229684
3504.473554	499205.706618	44.234689
3504.345818	499181.580108	44.239693
3504.407010	499165.472632	44.244698
3504.650096	499140.831861	44.249703
3504.298344	499135.268421	44.254708
3504.309226	499121.345614	44.259713
3503.952062	499118.921606	44.264717
3504.408997	499099.663566	44.269722
3504.197198	499075.702066	44.274727
3503.653562	499069.763953	44.279732
3504.188795	499055.910091	44.284737
3504.070694	499061.800999	44.289741
3503.911597	499056.713311	44.294746
3504.360653	499031.989216	44.299751
3504.384427	499018.469272	44.304756
3504.242899	499018.086696	44.309761
3503.997875	498998.585131	44.314765
3504.343103	498979.293994	44.319770
3504.413118	498971.335201	44.324775
3504.111736	498955.588577	44.329780
3504.330100	498934.545646	44.334785
3504.378361	498920.313039	44.339789
3504.167098	498920.852693	44.344794
3504.005769	498889.087047	44.349799
3504.023727	498870.454993	44.354804
3504.047284	498862.959101	44.359809
3504.016998	498887.364202	44.364813
3504.206288	498857.213643	44.369818
3503.996011	498839.174481	44.374823
3503.996627	498840.490620	44.379828
3504.235702	498820.659237	44.384833
3503.729687	498824.485359	44.389837
3503.981763	498820.395705	44.394842
3504.143610	498797.336621	44.399847
3503.970418	498773.419240	44.404852
3503.970340	498774.836740	44.409857
3503.762195	498772.237263	44.414861
3503.975163	498770.128087	44.419866
3504.241283	498762.796311	44.424871
3503.885488	498745.640650	44.429876
3504.346884	498727.849585	44.434881
3504.175498	498736.634554	44.439885
3504.094039	498715.486883	44.444890
3504.283355	498693.840781	44.449895
3504.297120	498693.585524	44.454900
3504.274978	498681.287548	44.459905
3504.035452	498671.808215	44.464909
3504.047956	498666.187060	44.469914
3503.962086	498655.519091	44.474919
3503.852297	498648.499798	44.479924
3504.287895	498649.544710	44.484929
3504.047041	498631.003935	44.489933
3503.886548	498613.159173	44.494938
3504.077252	498601.434987	44.499943
3503.966570	498606.211149	44.504948
3504.203682	498589.670365	44.509953
3504.073976	498579.920508	44.514957
3503.985933	498566.215401	44.519962
3504.172978	498555.605488	44.524967
3503.895791	498552.561276	44.529972
3504.090120	498534.710982	44.534977
3503.895317	498524.870135	44.539981
3503.962174	498516.000409	44.544986
3504.104572	498509.751188	44.549991
3504.321593	498505.616380	44.554996
3504.193975	498488.272539	44.560001
3504.099935	498484.288137	44.565005
3503.809522	498463.628811	44.570010
3504.018030	498467.645824	44.575015
3503.972128	498471.095556	44.580020
3504.134426	498446.719725	44.585025
3503.991511	498421.227741	44.590029
3504.027558	498431.195056	44.595034
3503.953501	498427.308731	44.600039
3503.881341	498415.170351	44.605044
3504.072796	498387.752375	44.610049
3503.560650	498387.580233	44.615053
3503.926546	498389.496791	44.620058
3503.907227	498386.209297	44.625063
3504.047838	498379.504695	44.630068
3503.984517	498379.919734	44.635073
3504.200292	498371.026401	44.640077
3504.377352	498336.624455	44.645082
3504.006972	498338.404261	44.650087
3503.790506	498334.489799	44.655092
3504.210614	498327.994126	44.660097
3504.137986	498312.767655	44.665101
3504.027670	498301.799593	44.670106
3504.353800	498296.888125	44.675111
3504.175337	498276.210891	44.680116
3504.172050	498249.582854	44.685121
3503.949869	498242.935538	44.690125
3504.048632	498241.097475	44.695130
3504.083568	498243.572603	44.700135
3504.128378	498217.797538	44.705140
3504.404948	498203.173908	44.710145
3504.190913	498199.056532	44.715149
3504.154400	498180.685498	44.720154
3504.238802	498160.422212	44.725159
3504.079480	498159.789303	44.730164
3504.022800	498147.293921	44.735169
3504.422891	498135.688215	44.740173
3504.199089	498120.738600	44.745178
3504.140914	498114.622192	44.750183
3503.853477	498105.909510	44.755188
3504.296384	498079.109452	44.760193
3504.173563	498076.648264	44.765197
3504.279962	498071.467711	44.770202
3504.399176	498052.565683	44.775207
3503.877832	498044.497442	44.780212
3504.341449	498021.440299	44.785217
3503.977561	498017.498441	44.790221
3504.443668	498015.349170	44.795226
3503.957963	497993.150783	44.800231
3503.631278	497986.317388	44.805236
3504.182516	497972.257666	44.810241
3503.911596	497971.743640	44.815245
3503.871149	497969.775673	44.820250
3504.122757	497970.191574	44.825255
3503.939174	497950.628538	44.830260
3504.308929	497938.470619	44.835265
3504.097042	497954.198076	44.840269
3504.272607	497936.299532	44.845274
3504.166928	497911.661578	44.850279
3503.919133	497901.423761	44.855284
3504.092426	497894.561936	44.860289
3504.253112	497895.093460	44.865293
3504.017155	497869.767279	44.870298
3504.137313	497849.751122	44.875303
3503.905785	497843.662021	44.880308
3503.994147	497845.875631	44.885313
3503.796178	497844.945064	44.890317
3504.077927	497828.801536	44.895322
3504.016979	497810.433988	44.900327
3504.297818	497804.213270	44.905332
3504.201981	497789.344407	44.910337
3504.018532	497786.032119	44.915341
3503.878484	497768.537672	44.920346
3504.145756	497765.154145	44.925351
3504.335691	497754.593932	44.930356
3504.352848	497754.895014	44.935361
3503.912341	497728.132805	44.940365
3504.225111	497722.261396	44.945370
3504.129642	497716.960768	44.950375
3503.960638	497714.861213	44.955380
3503.896598	497682.824935	44.960385
3503.759066	497688.415603	44.965389
3503.748193	497659.357832	44.970394
3504.096043	497655.708418	44.975399
3504.266988	497663.477902	44.980404
3504.216491	497649.209274	44.985409
3504.094180	497633.635698	44.990413
3504.049322	497623.163143	44.995418
3504.162755	497607.957297	45.000423
3504.271477	497601.156194	45.005428
3504.411536	497585.794242	45.010433
3504.319568	497573.607800	45.015437
3503.879271	497569.627293	45.020442
3504.379856	497542.766700	45.025447
3503.924203	497528.511384	45.030452
3504.241818	497527.954955	45.035457
3504.415938	497524.586107	45.040461
3504.308289	497499.137874	45.045466
3504.116986	497490.004685	45.050471
3503.999412	497485.922527	45.055476
3504.217660	497469.484955	45.060481
3504.181959	497456.530138	45.065485
3504.091160	497440.040129	45.070490
3504.197450	497427.113476	45.075495
3503.827247	497425.146940	45.080500
3504.041844	497397.470672	45.085505
3503.891972	497389.799070	45.090509
3504.330241	497384.262108	45.095514
3504.412822	497378.781359	45.100519
3504.274269	497363.767015	45.105524
3504.218676	497343.929958	45.110529
3504.270546	497344.478697	45.115533
3504.128076	497327.490479	45.120538
3504.273389	497303.217047	45.125543
3504.169082	497306.878741	45.130548
3504.140465	497299.643584	45.135553
3504.180647	497272.652847	45.140557
3504.040449	497269.941158	45.145562
3504.113790	497257.576494	45.150567
3503.838134	497253.164875	45.155572
3504.034627	497250.703735	45.160577
3504.107675	497234.035761	45.165581
3504.050369	497217.742766	45.170586
3504.087995	497205.383711	45.175591
3504.185530	497204.457035	45.180596
3504.016442	497187.928542	45.185601
3503.707879	497170.409522	45.190605
3503.497789	497150.191649	45.195610
3503.953049	497153.714307	45.200615
3503.736109	497151.470379	45.205620
3503.922158	497145.213790	45.210625
3504.246723	497154.376792	45.215629
3503.874833	497132.817520	45.220634
3503.608192	497116.962543	45.225639
3503.711416	497114.060474	45.230644
3503.806194	497105.286900	45.235649
3503.646915	497107.438483	45.240653
3503.601640	497107.091280	45.245658
3504.131681	497099.514610	45.250663
3504.011760	497106.267116	45.255668
3504.036970	497108.288285	45.260673
3504.259997	497074.484212	45.265677
3504.119858	497062.507551	45.270682
3503.935298	497069.422172	45.275687
3503.948612	497059.091981	45.280692
3504.190068	497049.890174	45.285697
3504.379710	497040.089013	45.290701
3503.969465	497026.332405	45.295706
3504.270780	497025.474770	45.300711
3503.983537	497007.294056	45.305716
3504.193539	496975.820756	45.310721
3503.787664	496974.112949	45.315725
3503.881840	496977.642082	45.320730
3504.191843	496969.948250	45.325735
3503.838601	496961.903582	45.330740
3504.309126	496933.122963	45.335745
3504.226197	496935.718156	45.340749
3503.856380	496922.410735	45.345754
3504.054392	496919.544283	45.350759
3503.876726	496897.346493	45.355764
3504.039400	496892.966766	45.360769
3503.735081	496877.876962	45.365773
3503.860093	496881.198726	45.370778
3504.118307	496877.613953	45.375783
3504.023549	496879.147823	45.380788
3504.074642	496860.305947	45.385793
3504.035332	496837.630559	45.390797
3503.765174	496845.773881	45.395802
3504.130132	496837.716907	45.400807
3504.229288	496834.967323	45.405812
3504.503076	496822.975713	45.410817
3504.193493	496797.507782	45.415821
3504.189572	496787.028275	45.420826
3504.281627	496777.951200	45.425831
3504.015111	496771.715380	45.430836
3503.959652	496745.346522	45.435841
3504.074823	496745.227098	45.440845
3503.970007	496735.421683	45.445850
3504.211362	496711.182910	45.450855
3503.997655	496698.660717	45.455860
3504.494237	496690.836021	45.460865
3504.369177	496694.298600	45.465869
3504.040397	496665.643886	45.470874
3504.417052	496658.850714	45.475879
3504.087878	496657.687674	45.480884
3504.412210	496634.296382	45.485889
3504.229321	496620.959196	45.490893
3504.330566	496608.083387	45.495898
3504.404508	496587.212444	45.500903
3504.229816	496564.304965	45.505908
3504.493419	496569.326284	45.510913
3504.265768	496553.565910	45.515917
3504.039270	496532.894276	45.520922
3504.355665	496519.629995	45.525927
3503.814917	496517.234645	45.530932
3504.213661	496507.349521	45.535937
3504.063831	496498.664944	45.540941
3503.745527	496480.083574	45.545946
3504.336404	496469.560507	45.550951
3504.164351	496480.625010	45.555956
3504.072919	496460.033206	45.560961
3503.948737	496443.496937	45.565965
3503.732165	496440.695934	45.570970
3503.905825	496423.150609	45.575975
3503.650229	496434.228343	45.580980
3503.728765	496424.748190	45.585985
3503.918473	496421.174155	45.590989
3503.543595	496406.044481	45.595994
3503.781049	496377.907379	45.600999
3503.485820	496392.079831	45.606004
3503.967178	496377.574256	45.611009
3503.830524	496375.823841	45.616013
3503.630968	496386.791487	45.621018
3504.059552	496387.381977	45.626023
3504.033826	496392.854112	45.631028
3503.909545	496367.609441	45.636033
3504.203032	496341.589888	45.641037
3504.138317	496338.106678	45.646042
3504.178967	496330.657667	45.651047
3504.259951	496335.505393	45.656052
3503.947045	496309.379112	45.661057
3503.997829	496299.548869	45.666061
3504.043366	496292.605372	45.671066
3504.265840	496280.520256	45.676071
3503.608341	496283.206349	45.681076
3503.883649	496263.214554	45.686081
3503.905217	496247.971460	45.691085
3503.739990	496252.807490	45.696090
3504.045173	496241.975034	45.701095
3503.953188	496248.166509	45.706100
3504.011934	496244.309356	45.711105
3504.229186	496233.490792	45.716109
3503.844182	496219.780212	45.721114
3503.834455	496210.820202	45.726119
3503.800518	496198.674295	45.731124
3503.792027	496204.295654	45.736129
3503.992454	496194.289813	45.741133
3503.971983	496197.179022	45.746138
3504.084356	496166.175426	45.751143
3503.887115	496163.826999	45.756148
3503.986647	496149.432221	45.761153
3504.118826	496157.714783	45.766157
3504.132667	496150.067414	45.771162
3504.285968	496121.285019	45.776167
3504.179214	496118.213456	45.781172
3503.961171	496112.577316	45.786177
3504.146468	496100.497956	45.791181
3504.094293	496082.127272	45.796186
3504.163875	496072.293936	45.801191
3504.046577	496063.047070	45.806196
3503.909496	496062.258678	45.811201
3504.015569	496050.293068	45.816205
3504.011089	496040.977729	45.821210
3504.078157	496005.525501	45.826215
3504.118580	496017.721215	45.831220
3503.688630	496008.827521	45.836225
3503.733390	496005.276314	45.841229
3503.689268	496003.815024	45.846234
3504.052154	495982.442043	45.851239
3503.569972	495980.543675	45.856244
3503.607307	495955.019734	45.861249
3503.930056	495966.613920	45.866253
3503.644661	495968.734937	45.871258
3503.991397	495966.452405	45.876263
3503.905152	495962.364952	45.881268
3503.499940	495955.543197	45.886273
3504.026636	495955.561254	45.891277
3503.910767	495955.225185	45.896282
3503.656660	495930.506739	45.901287
3503.927547	495918.160575	45.906292
3504.117046	495920.915380	45.911297
3504.116426	495915.244815	45.916301
3503.628838	495930.713807	45.921306
3503.844928	495925.768463	45.926311
3503.773414	495900.312281	45.931316
3503.844874	495896.807464	45.936321
3503.906878	495881.051359	45.941325
3503.807250	495877.624210	45.946330
3503.901969	495873.052454	45.951335
3503.731680	495877.332439	45.956340
3504.097481	495868.312909	45.961345
3503.996091	495855.215438	45.966349
3503.711214	495848.323993	45.971354
3504.004056	495834.354097	45.976359
3503.765362	495837.227221	45.981364
3503.831550	495840.760999	45.986369
3503.993881	495827.723090	45.991373
3504.067898	495824.774802	45.996378
3503.865037	495802.782184	46.001383
3503.597771	495798.318251	46.006388
3504.058911	495789.131721	46.011393
3504.090062	495781.835882	46.016397
3503.774390	495793.126026	46.021402
3503.957599	495781.046785	46.026407
3503.916552	495772.395299	46.031412
3504.017621	495760.734080	46.036417
3504.004711	495755.014776	46.041421
3503.891783	495748.956856	46.046426
3504.058524	495754.550659	46.051431
3503.871751	495759.440856	46.056436
3503.881509	495726.022410	46.061441
3504.239155	495726.826662	46.066445
3503.664450	495711.019145	46.071450
3503.951879	495701.454971	46.076455
3503.986372	495691.626976	46.081460
3504.009352	495696.078984	46.086465
3503.895499	495656.300332	46.091469
3504.002707	495655.270785	46.096474
3504.196207	495660.505964	46.101479
3504.020404	495660.483153	46.106484
3504.078432	495636.828880	46.111489
3504.285844	495616.239523	46.116493
3503.797297	495608.165007	46.121498
3503.870963	495602.583868	46.126503
3503.904595	495603.236807	46.131508
3503.777573	495603.661976	46.136513
3503.694812	495602.206761	46.141517
3503.810485	495576.011692	46.146522
3504.470509	495567.350572	46.151527
3504.089197	495570.195645	46.156532
3504.034867	495568.381509	46.161537
3504.282805	495550.621077	46.166541
3503.747475	495536.224889	46.171546
3504.151797	495524.211797	46.176551
3504.173800	495523.499503	46.181556
3504.264543	495511.029639	46.186561
3503.854694	495492.562994	46.191565
3503.760213	495483.869184	46.196570
3504.175230	495469.575906	46.201575
3503.797259	495482.546959	46.206580
3503.697991	495476.993114	46.211585
3503.758348	495474.806415	46.216589
3503.617877	495470.929952	46.221594
3503.909967	495458.732025	46.226599
3503.974887	495441.405473	46.231604
3503.782267	495432.372722	46.236609
3503.721204	495417.344524	46.241613
3503.695269	495429.146059	46.246618
3503.908494	495423.795972	46.251623
3503.708279	495427.220037	46.256628
3503.411632	495427.722651	46.261633
3503.806931	495416.723567	46.266637
3503.608738	495425.311839	46.271642
3503.693532	495416.792194	46.276647
3503.728310	495400.837449	46.281652
3503.844123	495393.730605	46.286657
3503.946144	495388.853779	46.291661
3503.745379	495384.885561	46.296666
3504.214155	495368.558399	46.301671
3503.730570	495381.444949	46.306676
3504.079744	495381.794862	46.311681
3503.871111	495356.207694	46.316685
3504.000008	495340.035489	46.321690
3504.088395	495331.768401	46.326695
3503.871313	495340.815394	46.331700
3503.685744	495342.616909	46.336705
3504.001142	495336.237992	46.341709
3503.731673	495312.331262	46.346714
3504.026938	495295.322596	46.351719
3503.721728	495292.029094	46.356724
3503.649903	495292.040482	46.361729
3504.047491	495289.597932	46.366733
3503.723932	495305.244057	46.371738
3503.882437	495288.510165	46.376743
3503.763653	495285.946693	46.381748
3503.755123	495258.403708	46.386753
3504.104281	495253.082722	46.391757
3503.824776	495257.987708	46.396762
3503.893021	495231.192045	46.401767
3504.026002	495247.120498	46.406772
3503.642310	495246.928010	46.411777
3503.987684	495238.164566	46.416781
3503.948433	495236.601179	46.421786
3504.149863	495209.885702	46.426791
3504.420758	495205.437835	46.431796
3504.436847	495189.637758	46.436801
3504.448058	495168.572575	46.441805
3503.855258	495156.767468	46.446810
3504.249212	495156.350808	46.451815
3503.823609	495126.949476	46.456820
3503.764609	495124.933500	46.461825
3503.806988	495112.015307	46.466829
3503.639415	495118.826712	46.471834
3503.717449	495122.763825	46.476839
3503.849855	495112.666877	46.481844
3503.908574	495119.290616	46.486849
3504.109718	495115.157553	46.491853
3503.961778	495109.307488	46.496858
3504.211372	495071.951163	46.501863
3504.109438	495074.549622	46.506868
3504.133889	495066.646955	46.511873
3504.163812	495058.996587	46.516877
3503.952170	495053.156572	46.521882
3504.071226	495032.276721	46.526887
3503.916577	495034.377181	46.531892
3504.082281	495040.275169	46.536897
3504.241831	495023.540870	46.541901
3503.914399	495007.086056	46.546906
3504.197892	494996.205659	46.551911
3504.202134	494990.128969	46.556916
3503.938537	494975.993194	46.561921
3504.133744	494953.329033	46.566925
3504.328807	494943.222090	46.571930
3504.171284	494940.816593	46.576935
3504.240948	494939.084065	46.581940
3503.973276	494900.745830	46.586945
3504.197938	494894.836808	46.591949
3503.664280	494888.034952	46.596954
3503.951147	494887.230139	46.601959
3503.865303	494900.256701	46.606964
3503.678934	494880.488264	46.611969
3503.930440	494855.739087	46.616973
3503.948834	494847.837282	46.621978
3504.024163	494844.483556	46.626983
3503.554113	494857.115163	46.631988
3503.695708	494847.016616	46.636993
3504.045265	494851.214679	46.641997
3503.881686	494845.012562	46.647002
3503.940266	494818.622897	46.652007
3504.152313	494807.146068	46.657012
3503.635230	494808.139246	46.662017
3503.850008	494803.598883	46.667021
3503.875143	494801.620208	46.672026
3503.896328	494796.452194	46.677031
3503.744167	494803.008108	46.682036
3503.594876	494782.119750	46.687041
3503.608518	494753.256008	46.692045
3503.662366	494763.779500	46.697050
3503.581587	494753.310972	46.702055
3503.581827	494751.083054	46.707060
3503.376158	494756.128408	46.712065
3503.567334	494757.921070	46.717069
3503.465660	494758.544790	46.722074
3503.822244	494747.348887	46.727079
3503.922501	494753.054773	46.732084
3503.897684	494768.856678	46.737089
3503.828109	494746.791090	46.742093
3503.681555	494750.865047	46.747098
3503.696774	494754.103284	46.752103
3503.658742	494753.856159	46.757108
3503.623788	494724.898784	46.762113
3503.968209	494710.616074	46.767117
3503.980739	494703.373383	46.772122
3503.953585	494694.871096	46.777127
3503.880881	494719.946746	46.782132
3503.907472	494702.473650	46.787137
3503.821814	494689.271588	46.792141
3503.761344	494678.090922	46.797146
3503.735444	494670.854292	46.802151
3504.014384	494655.164117	46.807156
3503.921540	494652.849629	46.812161
3504.156260	494654.483515	46.817165
3504.053599	494663.563393	46.822170
3503.952570	494639.477258	46.827175
3504.152169	494628.508633	46.832180
3503.849207	494620.860059	46.837185
3504.288726	494603.929225	46.842189
3503.891401	494605.409833	46.847194
3503.758766	494595.354490	46.852199
3503.988293	494564.987920	46.857204
3503.810961	494568.864242	46.862209
3504.008829	494574.757297	46.867213
3503.863789	494566.729297	46.872218
3504.239964	494562.872256	46.877223
3503.912106	494548.645037	46.882228
3503.810877	494528.660225	46.887233
3503.954393	494527.675512	46.892237
3504.092646	494522.640824	46.897242
3504.085141	494521.072359	46.902247
3504.220263	494502.113500	46.907252
3503.989287	494514.808827	46.912257
3504.096165	494482.638641	46.917261
3503.937606	494483.068819	46.922266
3504.019441	494487.258643	46.927271
3503.917963	494449.298280	46.932276
3504.131722	494445.669426	46.937281
3504.259198	494438.611005	46.942285
3503.972835	494443.466657	46.947290
3503.739388	494444.718836	46.952295
3504.082852	494403.092948	46.957300
3503.920108	494399.422319	46.962305
3504.147785	494398.120486	46.967309
3503.682148	494392.674850	46.972314
3504.317205	494393.992311	46.977319
3504.110585	494383.391555	46.982324
3503.903274	494353.903845	46.987329
3503.980975	494349.486306	46.992333
3503.821112	494354.423259	46.997338
3503.972390	494340.727779	47.002343
3504.089599	494331.189795	47.007348
3504.004710	494324.418073	47.012353
3504.174224	494320.745551	47.017357
3504.016108	494320.821213	47.022362
3504.073408	494315.039728	47.027367
3504.134127	494289.205956	47.032372
3503.712026	494275.702320	47.037377
3504.249464	494265.135807	47.042381
3503.977838	494265.381316	47.047386
3503.791034	494266.524864	47.052391
3503.743905	494264.557553	47.057396
3503.707730	494246.942035	47.062401
3503.766261	494218.728625	47.067405
3503.747904	494217.465665	47.072410
3503.729255	494211.898694	47.077415
3503.899562	494219.365934	47.082420
3503.612723	494224.626806	47.087425
3503.957836	494221.635414	47.092429
3503.922170	494212.425346	47.097434
3503.799634	494215.229726	47.102439
3503.579289	494205.491847	47.107444
3503.407584	494183.441723	47.112449
3503.783382	494179.837843	47.117453
3503.626569	494184.267999	47.122458
3503.687354	494163.396371	47.127463
3503.576348	494166.452117	47.132468
3503.662929	494168.514549	47.137473
3503.729735	494166.681128	47.142477
3504.052467	494165.009803	47.147482
3504.068129	494160.298208	47.152487
3503.838175	494159.423138	47.157492
3503.702775	494157.672310	47.162497
3503.553033	494131.770308	47.167501
3503.428793	494144.752838	47.172506
3503.692612	494124.760528	47.177511
3503.763586	494131.483960	47.182516
3503.624385	494129.480549	47.187521
3503.832889	494122.105384	47.192525
3504.020631	494124.354378	47.197530
3503.748453	494134.929757	47.202535
3503.565510	494128.325368	47.207540
3503.698308	494114.784550	47.212545
3503.579491	494114.803365	47.217549
3503.930533	494127.508244	47.222554
3503.903715	494115.967465	47.227559
3503.955704	494091.653882	47.232564
3503.724940	494089.158576	47.237569
3504.042067	494074.778414	47.242573
3503.683908	494078.936599	47.247578
3504.100140	494074.819945	47.252583
3504.188584	494078.806274	47.257588
3504.013119	494058.022501	47.262593
3504.177773	494040.830774	47.267597
3503.966724	494042.636441	47.272602
3503.950182	494028.815343	47.277607
3504.019277	494029.209551	47.282612
3503.677495	494011.085107	47.287617
3504.003345	493991.082849	47.292621
3503.762355	493991.424792	47.297626
3503.673304	493989.058984	47.302631
3503.683987	493985.563409	47.307636
3503.787126	493991.015895	47.312641
3504.048178	493985.657832	47.317645
3503.960054	493985.367977	47.322650
3503.709787	493953.253311	47.327655
3504.037722	493954.771255	47.332660
3503.834294	493951.360149	47.337665
3504.089239	493944.180120	47.342669
3504.024524	493948.291957	47.347674
3504.144716	493932.018615	47.352679
3503.886125	493920.109250	47.357684
3503.885388	493912.716434	47.362689
3504.321129	493900.241588	47.367693
3503.776855	493895.922242	47.372698
3503.886577	493891.398259	47.377703
3504.306822	493876.140819	47.382708
3504.081164	493861.795641	47.387713
3504.005070	493866.061205	47.392717
3503.950781	493861.968231	47.397722
3504.056473	493828.429892	47.402727
3504.077298	493821.590640	47.407732
3503.925182	493814.474895	47.412737
3504.121306	493799.911096	47.417741
3503.944724	493823.535909	47.422746
3503.904291	493795.286854	47.427751
3504.043449	493771.161621	47.432756
3503.858458	493767.342469	47.437761
3504.045524	493762.704957	47.442765
3504.077108	493771.207048	47.447770
3503.884099	493754.223492	47.452775
3504.234921	493729.609017	47.457780
3504.001383	493727.519197	47.462785
3504.339496	493712.983526	47.467789
3504.008180	493712.225728	47.472794
3504.171048	493681.918875	47.477799
3504.290328	493680.634125	47.482804
3504.243692	493677.603287	47.487809
3504.376049	493655.555111	47.492813
3504.070841	493644.665684	47.497818
3503.870206	493618.669729	47.502823
3503.785150	493609.619078	47.507828
3503.448813	493619.951704	47.512833
3503.721443	493615.401907	47.517837
3503.751783	493614.080571	47.522842
3503.718790	493607.148469	47.527847
3504.093258	493610.937781	47.532852
3503.899814	493599.676200	47.537857
3503.705417	493594.288732	47.542861
3503.566225	493591.323146	47.547866
3503.832231	493585.103345	47.552871
3503.915728	493590.255228	47.557876
3503.827154	493583.686365	47.562881
3504.024348	493567.501808	47.567885
3503.956418	493557.182481	47.572890
3503.617535	493549.539136	47.577895
3503.906290	493535.112402	47.582900
3503.632943	493547.460625	47.587905
3503.792073	493539.586654	47.592909
3503.541410	493536.233573	47.597914
3503.619253	493530.651147	47.602919
3503.939284	493534.651629	47.607924
3503.964118	493540.724278	47.612929
3503.881067	493528.635002	47.617933
3503.599922	493514.197046	47.622938
3503.620338	493503.863727	47.627943
3503.689702	493491.193320	47.632948
3503.832667	493486.613347	47.637953
3503.854184	493491.066122	47.642957
3503.720538	493493.619177	47.647962
3503.907805	493487.411788	47.652967
3503.969390	493485.579125	47.657972
3503.732470	493479.438775	47.662977
3503.799488	493458.616002	47.667981
3503.920046	493458.242519	47.672986
3503.523752	493451.519691	47.677991
3503.837585	493446.558236	47.682996
3503.794275	493445.451081	47.688001
3503.778475	493437.148970	47.693005
3503.888531	493442.246059	47.698010
3504.123658	493443.576162	47.703015
3503.916565	493420.720508	47.708020
3503.650781	493419.395321	47.713025
3503.713662	493406.422052	47.718029
3503.748724	493395.731890	47.723034
3503.819097	493397.037398	47.728039
3503.941968	493399.803116	47.733044
3503.643343	493399.192052	47.738049
3504.091371	493393.095334	47.743053
3503.898930	493380.314314	47.748058
3503.739791	493359.476535	47.753063
3504.259441	493348.962950	47.758068
3503.861498	493359.609288	47.763073
3504.226211	493346.537635	47.768077
3504.134254	493339.716029	47.773082
3503.737729	493316.890185	47.778087
3503.937770	493308.098158	47.783092
3503.892870	493313.827433	47.788097
3503.646486	493302.725954	47.793101
3503.612557	493304.807529	47.798106
3503.637766	493309.361041	47.803111
3503.948234	493295.892819	47.808116
3504.014038	493294.312662	47.813121
3503.903271	493269.162865	47.818125
3503.681773	493263.070643	47.823130
3503.781862	493266.498283	47.828135
3503.943766	493254.420751	47.833140
3503.958366	493256.697217	47.838145
3504.066385	493250.958021	47.843149
3503.806725	493240.668819	47.848154
3503.852297	493227.343690	47.853159
3504.109800	493213.124199	47.858164
3503.959494	493221.300819	47.863169
3503.950035	493222.061931	47.868173
3503.950074	493217.605757	47.873178
3503.960009	493189.297176	47.878183
3504.285774	493180.181385	47.883188
3503.817275	493170.532816	47.888193
3503.883673	493158.875427	47.893197
3503.737596	493163.810518	47.898202
3503.945989	493168.942779	47.903207
3504.069500	493140.362978	47.908212
3503.534987	493127.585208	47.913217
3503.753181	493124.512423	47.918221
3504.023078	493124.419164	47.923226
3503.775798	493123.850616	47.928231
3503.976573	493125.338089	47.933236
3503.810404	493130.023170	47.938241
3504.111624	493113.163467	47.943245
3503.768557	493098.886890	47.948250
3503.974656	493083.763921	47.953255
3503.892622	493087.220378	47.958260
3503.791049	493087.692219	47.963265
3503.921516	493075.467622	47.968269
3503.995164	493076.873913	47.973274
3503.931381	493048.880602	47.978279
3503.923761	493037.994422	47.983284
3503.620500	493035.864903	47.988289
3503.832687	493032.084104	47.993293
3503.663519	493035.301146	47.998298
3503.614736	493035.207614	48.003303
3503.765595	493029.107105	48.008308
3503.749301	493034.528111	48.013313
3503.818379	493033.048693	48.018317
3503.744854	493016.653244	48.023322
3503.845180	492996.938750	48.028327
3503.897109	492990.752585	48.033332
3503.509722	492985.091604	48.038337
3503.797756	492979.982184	48.043341
3503.685840	492982.835712	48.048346
3503.879554	492989.641441	48.053351
3504.102126	492981.200173	48.058356
3503.822414	492987.371775	48.063361
3503.965314	492970.233129	48.068365
3503.858314	492945.386132	48.073370
3503.824359	492951.620184	48.078375
3504.004414	492959.187675	48.083380
3503.805532	492945.090747	48.088385
3503.929090	492938.589407	48.093389
3503.679348	492926.880558	48.098394
3503.513392	492908.777879	48.103399
3503.787326	492897.188804	48.108404
3503.893974	492890.993957	48.113409
3503.706776	492905.709053	48.118413
3503.845654	492903.205802	48.123418
3503.728570	492888.893346	48.128423
3504.159445	492888.217609	48.133428
3504.199559	492890.439447	48.138433
3504.198064	492873.120974	48.143437
3504.196692	492864.158011	48.148442
3503.893816	492859.547067	48.153447
3504.170422	492856.566286	48.158452
3504.127458	492833.734605	48.163457
3504.214608	492822.276283	48.168461
3503.930789	492814.421371	48.173466
3504.166150	492814.131010	48.178471
3504.399592	492798.395810	48.183476
3503.923067	492782.874084	48.188481
3504.272974	492773.247879	48.193485
3504.203315	492768.397494	48.198490
3503.930208	492744.943758	48.203495
3504.243191	492729.246567	48.208500
3503.924399	492729.448908	48.213505
3504.185909	492731.939615	48.218509
3504.053534	492728.770251	48.223514
3504.219810	492702.157976	48.228519
3504.178818	492673.806014	48.233524
3503.833357	492690.369340	48.238529
3504.017826	492677.325704	48.243533
3504.032071	492653.877077	48.248538
3503.668244	492642.895042	48.253543
3503.864459	492632.938573	48.258548
3503.894064	492628.933348	48.263553
3503.855925	492626.002275	48.268557
3503.897417	492627.717524	48.273562
3503.632510	492631.709371	48.278567
3503.889477	492620.831769	48.283572
3503.702994	492606.935186	48.288577
3503.910303	492594.090442	48.293581
3503.958113	492584.967650	48.298586
3503.785646	492584.640461	48.303591
3503.774641	492584.895439	48.308596
3503.660814	492576.405873	48.313601
3503.734136	492578.622501	48.318605
3503.677089	492588.202594	48.323610
3503.776387	492571.627515	48.328615
3504.037742	492549.355072	48.333620
3503.569996	492545.529714	48.338625
3503.815198	492541.085271	48.343629
3504.089406	492539.522753	48.348634
3503.762805	492535.421883	48.353639
3504.055543	492529.197505	48.358644
3503.748884	492521.143515	48.363649
3503.932032	492510.733281	48.368653
3503.923936	492504.050034	48.373658
3503.630278	492482.624838	48.378663
3504.105168	492494.045255	48.383668
3503.736803	492496.584903	48.388673
3503.933610	492486.678903	48.393677
3503.933767	492485.210335	48.398682
3503.724687	492465.999944	48.403687
3503.985656	492447.474854	48.408692
3503.727317	492445.945856	48.413697
3503.974208	492437.044730	48.418701
3503.854891	492434.025175	48.423706
3503.948480	492434.010420	48.428711
3504.340759	492429.795909	48.433716
3503.814175	492421.776634	48.438721
3503.879932	492403.181072	48.443725
3504.064358	492396.214153	48.448730
3504.021139	492395.917175	48.453735
3504.283670	492384.835992	48.458740
3503.991991	492369.588550	48.463745
3504.035175	492349.122783	48.468749
3504.113819	492347.388594	48.473754
3503.858626	492357.861020	48.478759
3504.185179	492325.399153	48.483764
3504.039231	492313.369664	48.488769
3504.010129	492318.894185	48.493773
3503.761089	492311.185485	48.498778
3503.745223	492302.984159	48.503783
3504.020233	492300.206106	48.508788
3503.928085	492292.725808	48.513793
3503.955931	492271.452120	48.518797
3503.881878	492263.766386	48.523802
3503.859170	492257.389207	48.528807
3503.916093	492258.190508	48.533812
3503.779246	492268.441715	48.538817
3503.836472	492256.126871	48.543821
3503.920018	492223.551308	48.548826
3503.959665	492217.620033	48.553831
3504.017124	492211.280810	48.558836
3503.815350	492214.857637	48.563841
3504.015181	492207.331157	48.568845
3503.834400	492214.854699	48.573850
3503.568739	492192.462556	48.578855
3503.921012	492171.340045	48.583860
3503.695522	492166.868621	48.588865
3503.953228	492172.904914	48.593869
3503.506479	492161.631849	48.598874
3503.814646	492159.557517	48.603879
3503.958202	492158.825883	48.608884
3503.664574	492161.404406	48.613889
3503.828513	492162.695213	48.618893
3503.911412	492148.502502	48.623898
3503.491704	492143.403428	48.628903
3503.654568	492134.616721	48.633908
3503.683688	492134.510872	48.638913
3503.720696	492127.516511	48.643917
3503.946899	492132.241113	48.648922
3503.645752	492132.288744	48.653927
3503.982693	492123.322595	48.658932
3503.938394	492134.470799	48.663937
3504.035434	492132.075341	48.668941
3503.985329	492100.128385	48.673946
3503.752873	492090.391302	48.678951
3504.134393	492078.430221	48.683956
3503.997614	492080.983965	48.688961
3504.064470	492080.973435	48.693965
3503.547112	492066.571680	48.698970
3503.673898	492038.090946	48.703975
3503.874939	492039.173331	48.708980
3503.880342	492037.349404	48.713985
3504.054107	492032.612279	48.718989
3504.081591	492024.859756	48.723994
3503.942791	492031.110688	48.728999
3504.103795	492009.005384	48.734004
3503.920368	492005.033693	48.739009
3503.756543	491989.715089	48.744013
3503.866751	491978.759023	48.749018
3503.759788	491984.549160	48.754023
3504.193396	491973.086200	48.759028
3503.718038	491979.846120	48.764033
3503.785568	491950.969481	48.769037
3503.799686	491939.420873	48.774042
3503.912137	491948.164232	48.779047
3504.122696	491938.306409	48.784052
3503.887922	491945.686666	48.789057
3503.466486	491937.194782	48.794061
3504.003934	491933.564923	48.799066
3503.863626	491915.204009	48.804071
3504.049925	491902.868532	48.809076
3503.843667	491892.671424	48.814081
3503.888140	491902.843532	48.819085
3503.818983	491895.967148	48.824090
3503.425834	491890.813163	48.829095
3504.153105	491888.773848	48.834100
3504.014420	491862.259210	48.839105
3503.965138	491852.796906	48.844109
3503.938796	491845.913736	48.849114
3503.818259	491846.641818	48.854119
3504.057687	491844.932813	48.859124
3503.710450	491851.216748	48.864129
3503.831405	491823.344316	48.869133
3504.203601	491810.321045	48.874138
3503.992237	491809.442921	48.879143
3503.847836	491794.121086	48.884148
3504.112119	491788.609954	48.889153
3503.971123	491788.379062	48.894157
3503.984166	491761.688372	48.899162
3504.095334	491755.289862	48.904167
3504.042225	491749.727597	48.909172
3503.823001	491745.255081	48.914177
3503.851168	491748.491799	48.919181
3504.191042	491733.498517	48.924186
3503.836230	491726.262074	48.929191
3504.033792	491704.454487	48.934196
3503.789387	491708.392648	48.939201
3503.956736	491704.517382	48.944205
3504.101211	491704.292013	48.949210
3503.596226	491689.179009	48.954215
3503.930301	491677.275813	48.959220
3503.907141	491673.481292	48.964225
3503.966213	491666.280699	48.969229
3503.826946	491666.910461	48.974234
3503.555732	491670.650295	48.979239
3504.102112	491660.131535	48.984244
3504.096948	491652.485303	48.989249
3503.845198	491621.987397	48.994253
3503.785630	491625.896362	48.999258
3503.915024	491627.952313	49.004263
3504.005708	491619.683202	49.009268
3503.452107	491624.126035	49.014273
3503.699341	491607.425430	49.019277
3504.126854	491613.738927	49.024282
3503.824793	491595.555191	49.029287
3503.886305	491580.858996	49.034292
3503.752317	491584.881018	49.039297
3503.600080	491569.408306	49.044301
3503.604454	491570.724374	49.049306
3503.395731	491570.909329	49.054311
3503.791976	491566.693998	49.059316
3504.153477	491561.015505	49.064321
3503.848521	491561.772744	49.069325
3504.033577	491538.346356	49.074330
3503.859359	491527.384335	49.079335
3503.961963	491523.519264	49.084340
3503.819103	491525.162465	49.089345
3503.816979	491524.301901	49.094349
3503.975413	491524.124967	49.099354
3503.744559	491528.415527	49.104359
3504.120467	491499.641380	49.109364
3503.655281	491490.042051	49.114369
3503.830307	491486.874534	49.119373
3503.913705	491480.784179	49.124378
3503.717865	491477.270128	49.129383
3503.846041	491475.477386	49.134388
3503.610265	491483.111201	49.139393
3503.840144	491482.264611	49.144397
3504.090949	491449.711902	49.149402
3503.722939	491442.224217	49.154407
3503.936364	491426.440377	49.159412
3504.049293	491425.916130	49.164417
3503.826241	491429.141964	49.169421
3504.198978	491424.474525	49.174426
3504.170474	491409.792423	49.179431
3504.011386	491393.307775	49.184436
3503.883882	491395.100492	49.189441
3503.648960	491395.745381	49.194445
3503.870845	491390.240833	49.199450
3503.579643	491383.449996	49.204455
3503.884184	491376.109208	49.209460
3503.710225	491368.236317	49.214465
3503.736174	491348.886336	49.219469
3504.223148	491336.300389	49.224474
3503.575971	491341.720310	49.229479
3504.302057	491330.717169	49.234484
3504.142455	491334.945868	49.239489
3503.983802	491320.334909	49.244493
3503.996525	491307.418745	49.249498
3503.525676	491296.908620	49.254503
3504.194443	491287.636407	49.259508
3503.686967	491287.058277	49.264513
3503.682086	491283.412720	49.269517
3503.596301	491292.238362	49.274522
3503.519698	491294.428195	49.279527
3503.678501	491288.629724	49.284532
3503.835097	491289.972397	49.289537
3503.778023	491271.749625	49.294541
3503.979084	491251.916072	49.299546
3503.739250	491253.675911	49.304551
3503.754803	491250.077762	49.309556
3503.513298	491254.370068	49.314561
3503.426662	491256.257626	49.319565
3503.644144	491253.944309	49.324570
3503.816890	491247.586537	49.329575
3503.846161	491244.087506	49.334580
3503.505049	491246.471082	49.339585
3503.723225	491240.258059	49.344589
3503.657015	491240.623069	49.349594
3503.555216	491245.551670	49.354599
3503.613616	491215.004079	49.359604
3503.802335	491208.491837	49.364609
3503.605323	491215.613192	49.369613
3503.928045	491200.976703	49.374618
3503.582537	491213.185948	49.379623
3503.474075	491199.731776	49.384628
3503.698663	491209.116134	49.389633
3503.804345	491191.728511	49.394637
3504.141155	491198.461639	49.399642
3503.501647	491211.882167	49.404647
3503.917175	491197.433584	49.409652
3504.014611	491180.199186	49.414657
3503.679770	491157.259642	49.419661
3503.839004	491168.528189	49.424666
3503.710155	491166.978617	49.429671
3504.065592	491153.400450	49.434676
3503.547620	491167.460177	49.439681
3503.834691	491166.655179	49.444685
3504.096671	491149.445391	49.449690
3503.560685	491134.792634	49.454695
3503.784412	491111.308954	49.459700
3503.669915	491116.492818	49.464705
3503.889344	491109.013443	49.469709
3504.020676	491113.196211	49.474714
3503.832330	491107.503194	49.479719
3503.801804	491096.518208	49.484724
3504.038878	491119.574640	49.489729
3503.657583	491088.235380	49.494733
3503.579856	491075.991730	49.499738
3503.571655	491055.228795	49.504743
3503.947212	491059.575554	49.509748
3504.001829	491057.541175	49.514753
3503.981475	491059.620856	49.519757
3503.735023	491067.611040	49.524762
3503.393170	491063.208384	49.529767
3503.845637	491056.705049	49.534772
3503.642693	491065.853182	49.539777
3503.682795	491045.943561	49.544781
3503.780984	491024.404108	49.549786
3503.775527	491022.581799	49.554791
3503.680220	491023.052700	49.559796
3503.769308	491014.986152	49.564801
3503.654976	491023.715144	49.569805
3503.813788	491014.422104	49.574810
3503.506011	491009.963405	49.579815
3503.840359	491009.353507	49.584820
3503.752185	491012.304872	49.589825
3503.485793	491015.385693	49.594829
3503.920050	491004.833642	49.599834
3503.740075	491001.013125	49.604839
3503.783786	490980.697705	49.609844
3503.615800	490973.583375	49.614849
3503.767761	490967.076859	49.619853
3503.693188	490968.405446	49.624858
3503.346037	490971.397749	49.629863
3503.896347	490969.791466	49.634868
3503.557808	490975.871739	49.639873
3503.624199	490963.909107	49.644877
3504.074962	490958.722773	49.649882
3503.807273	490967.881187	49.654887
3503.760058	490980.600531	49.659892
3503.939352	490948.817923	49.664897
3503.579131	490929.528541	49.669901
3503.662761	490931.946316	49.674906
3503.639106	490938.078125	49.679911
3503.894545	490917.172079	49.684916
3503.792101	490930.355991	49.689921
3503.579721	490920.260607	49.694925
3503.580905	490921.982384	49.699930
3503.493098	490928.174981	49.704935
3503.411353	490917.907014	49.709940
3503.986858	490922.424784	49.714945
3503.814567	490925.946551	49.719949
3503.759713	490915.117238	49.724954
3503.572128	490910.487585	49.729959
3503.563742	490893.168357	49.734964
3503.861685	490877.471986	49.739969
3503.410415	490884.127202	49.744973
3503.707688	490877.040592	49.749978
3503.359927	490878.108493	49.754983
3503.484810	490878.139437	49.759988
3503.578455	490889.114649	49.764993
3503.872955	490879.901387	49.769997
3503.646490	490871.530134	49.775002
3503.715783	490876.685017	49.780007
3504.194792	490873.317417	49.785012
3504.140412	490874.744111	49.790017
3503.721182	490871.771701	49.795021
3503.741421	490837.025981	49.800026
3503.773549	490836.159972	49.805031
3503.879411	490830.521662	49.810036
3504.227101	490826.465776	49.815041
3503.774545	490829.373469	49.820045
3504.147630	490831.137768	49.825050
3503.792405	490812.505862	49.830055
3504.119073	490785.561627	49.835060
3504.150073	490782.923208	49.840065
3503.761951	490792.303323	49.845069
3504.085022	490785.364537	49.850074
3504.177093	490773.093852	49.855079
3503.447420	490751.634281	49.860084
3503.747758	490748.446835	49.865089
3503.952332	490746.388722	49.870093
3503.798556	490740.842065	49.875098
3503.506567	490740.938896	49.880103
3504.038882	490741.918355	49.885108
3503.739065	490745.966766	49.890113
3503.620477	490738.996475	49.895117
3504.215769	490724.924281	49.900122
3504.003885	490703.636046	49.905127
3503.987862	490694.724999	49.910132
3503.586350	490696.864962	49.915137
3504.033755	490691.071338	49.920141
3504.333134	490684.592070	49.925146
3503.897311	490684.610342	49.930151
3503.936061	490659.787900	49.935156
3503.948440	490659.735334	49.940161
3503.649685	490656.794494	49.945165
3503.938093	490655.229579	49.950170
3503.902125	490655.336591	49.955175
3503.969843	490648.640696	49.960180
3503.965034	490627.167710	49.965185
3503.912669	490620.794658	49.970189
3504.238542	490601.700376	49.975194
3503.679093	490608.676661	49.980199
3504.091762	490602.989792	49.985204
3504.206235	490576.078793	49.990209
3503.798335	490564.798616	49.995213
3503.832811	490563.223181	50.000218
3503.704103	490566.839419	50.005223
3503.794987	490558.265931	50.010228
3503.482888	490568.900291	50.015233
3503.606747	490558.143818	50.020237
3503.744305	490549.411011	50.025242
3503.493204	490545.145827	50.030247
3503.579640	490549.639693	50.035252
3503.805045	490530.257341	50.040257
3503.446467	490527.781750	50.045261
3503.668930	490515.388995	50.050266
3503.679653	490517.210595	50.055271
3503.694353	490518.069291	50.060276
3503.641439	490505.568114	50.065281
3503.444612	490509.245776	50.070285
3503.769779	490501.344279	50.075290
3503.751547	490505.905344	50.080295
3503.411906	490511.124959	50.085300
3504.059232	490508.389092	50.090305
3503.505735	490503.817169	50.095309
3503.864893	490505.482408	50.100314
3503.599830	490506.233382	50.105319
3503.822023	490501.842739	50.110324
3503.722435	490486.968561	50.115329
3503.628511	490470.472799	50.120333
3504.185914	490467.295323	50.125338
3503.579319	490462.174673	50.130343
3503.386153	490459.672930	50.135348
3503.686851	490451.825926	50.140353
3503.528643	490462.486669	50.145357
3503.771294	490461.587370	50.150362
3503.602970	490470.173214	50.155367
3503.590874	490459.742049	50.160372
3503.844335	490460.816243	50.165377
3503.284469	490474.123417	50.170381
3503.738528	490446.854684	50.175386
3503.504754	490471.708305	50.180391
3503.389793	490461.141460	50.185396
3503.711808	490460.229617	50.190401
3503.960608	490462.671995	50.195405
3503.823977	490450.133367	50.200410
3503.494860	490428.964640	50.205415
3503.681159	490411.563551	50.210420
3503.717857	490409.785166	50.215425
3503.491855	490423.495426	50.220429
3503.455323	490408.003464	50.225434
3503.570874	490412.999224	50.230439
3503.272545	490415.426788	50.235444
3503.704201	490410.395263	50.240449
3503.431008	490418.086071	50.245453
3503.800687	490403.492184	50.250458
3503.418199	490404.970770	50.255463
3503.510026	490400.347476	50.260468
3503.666818	490412.781731	50.265473
3503.192067	490416.098165	50.270477
3503.513860	490403.183175	50.275482
3503.362769	490419.515209	50.280487
3503.424790	490406.894509	50.285492
3503.709955	490410.242780	50.290497
3503.549660	490415.839246	50.295501
3503.803407	490408.252876	50.300506
3503.455552	490421.172055	50.305511
3503.788214	490409.825387	50.310516
3503.694210	490409.587049	50.315521
3503.384034	490417.942104	50.320525
3503.894119	490410.517807	50.325530
3503.607578	490411.221533	50.330535
3503.894381	490409.555558	50.335540
3503.793620	490407.849544	50.340545
3503.709192	490401.329546	50.345549
3503.792000	490382.526688	50.350554
3503.843861	490377.707119	50.355559
3503.754262	490371.745038	50.360564
3504.232651	490372.479810	50.365569
3503.701894	490369.524945	50.370573
3503.670997	490369.225986	50.375578
3504.079453	490371.187325	50.380583
3503.717616	490338.526923	50.385588
3503.721476	490327.333464	50.390593
3503.961437	490331.144713	50.395597
3503.910720	490316.262676	50.400602
3503.795504	490323.168856	50.405607
3504.003626	490326.174793	50.410612
3504.306380	490318.378055	50.415617
3503.852368	490299.761251	50.420621
3503.901425	490286.534759	50.425626
3503.867890	490281.374135	50.430631
3503.647595	490289.917629	50.435636
3503.853882	490285.580096	50.440641
3503.823714	490280.064413	50.445645
3503.705878	490271.321195	50.450650
3503.691010	490254.964689	50.455655
3503.760077	490230.086239	50.460660
3504.123208	490215.290654	50.465665
3503.471318	490239.248375	50.470669
3503.702819	490230.247339	50.475674
3504.024418	490225.537039	50.480679
3503.740643	490220.466595	50.485684
3503.803394	490230.788667	50.490689
3504.091191	490232.363916	50.495693
3503.895158	490202.563940	50.500698
3503.676544	490202.547881	50.505703
3503.995269	490200.927490	50.510708
3503.937016	490190.503470	50.515713
3503.837823	490196.546167	50.520717
3504.097864	490179.740971	50.525722
3504.069677	490170.274480	50.530727
3503.826794	490140.583104	50.535732
3503.974908	490116.806245	50.540737
3503.696425	490070.812005	50.545741
3504.084002	490019.293112	50.550746
3503.655215	489961.825399	50.555751
3503.404416	489895.719268	50.560756
3503.575956	489810.502535	50.565761
3503.284058	489735.792183	50.570765
3503.331902	489640.869783	50.575770
3503.121510	489532.211277	50.580775
3502.773578	489421.851814	50.585780
3502.682038	489295.749894	50.590785
3502.249152	489172.993306	50.595789
3502.285686	489029.395217	50.600794
3501.397275	488891.564418	50.605799
3501.592314	488738.467430	50.610804
3501.302447	488589.497938	50.615809
3500.924635	488430.765403	50.620813
3500.672433	488254.789966	50.625818
3500.532355	488063.650036	50.630823
3500.289652	487896.382017	50.635828
3500.076261	487693.245151	50.640833
3499.890771	487495.926928	50.645837
3499.548273	487280.851668	50.650842
3499.031572	487077.553533	50.655847
3498.795520	486850.856523	50.660852
3498.462673	486631.922553	50.665857
3497.860003	486398.794081	50.670861
3497.527051	486149.966896	50.675866
3497.015435	485922.846491	50.680871
3496.572251	485668.610020	50.685876
3496.506350	485418.565957	50.690881
3496.060639	485173.543376	50.695885
3495.692211	484909.507582	50.700890
3495.377538	484638.063053	50.705895
3494.213314	484354.741968	50.710900
3494.480963	484092.570271	50.715905
3493.960417	483820.792129	50.720909
3493.434334	483527.985224	50.725914
3492.972371	483245.600826	50.730919
3492.114135	482947.011115	50.735924
3491.742974	482653.609185	50.740929
3491.297116	482359.809291	50.745933
3491.202453	482055.917098	50.750938
3490.493306	481749.127804	50.755943
3489.954369	481442.610805	50.760948
3489.475815	481122.753015	50.765953
3488.566784	480807.214465	50.770957
3488.468185	480490.630639	50.775962
3487.606696	480169.196302	50.780967
3487.252930	479846.308262	50.785972
3486.491605	479518.969272	50.790977
3485.971639	479185.961682	50.795981
3485.623266	478859.661369	50.800986
3485.033144	478525.082769	50.805991
3484.430954	478186.648873	50.810996
3484.218348	477838.771963	50.816001
3483.313166	477499.766118	50.821005
3482.863231	477154.955594	50.826010
3482.489042	476802.626218	50.831015
3481.596612	476442.111246	50.836020
3481.129252	476106.002856	50.841025
3480.267185	475757.077344	50.846029
3479.733325	475391.722488	50.851034
3478.987957	475037.139962	50.856039
3477.970074	474693.086551	50.861044
3477.982871	474330.819393	50.866049
3477.143822	473973.952070	50.871053
3476.385183	473616.102655	50.876058
3475.694362	473261.480438	50.881063
3475.033765	472892.704275	50.886068
3474.356595	472543.035201	50.891073
3473.692080	472193.814390	50.896077
3473.167503	471826.163449	50.901082
3472.472801	471465.123204	50.906087
3472.145424	471107.111027	50.911092
3471.781052	470736.829788	50.916097
3470.820379	470370.742701	50.921101
3470.140822	470001.968357	50.926106
3469.727184	469623.157559	50.931111
3468.668081	469257.573364	50.936116
3468.316124	468881.477139	50.941121
3467.348526	468530.366370	50.946125
3466.961376	468139.913541	50.951130
3465.943754	467779.215116	50.956135
3465.074424	467424.115316	50.961140
3464.902660	467048.312604	50.966145
3463.891436	466687.442303	50.971149
3463.879360	466311.347675	50.976154
3462.708012	465940.703308	50.981159
3462.295817	465562.934527	50.986164
3461.862012	465175.527437	50.991169
3460.665262	464819.370702	50.996173
3460.167142	464430.743149	51.001178
3459.404183	464060.052148	51.006183
3458.163825	463697.899433	51.011188
3457.832033	463319.165344	51.016193
3457.038283	462955.306618	51.021197
3456.594695	462596.052321	51.026202
3455.762592	462227.064973	51.031207
3454.968139	461861.767813	51.036212
3454.776702	461486.732513	51.041217
3453.671750	461130.145089	51.046221
3453.220117	460750.218351	51.051226
3452.503010	460375.297691	51.056231
3451.628742	460012.061652	51.061236
3451.076990	459647.855575	51.066241
3450.355345	459277.938445	51.071245
3449.859836	458905.696701	51.076250
3449.184470	458546.006433	51.081255
3448.091446	458174.607675	51.086260
3447.609629	457799.352199	51.091265
3446.784518	457445.197005	51.096269
3446.186424	457067.766192	51.101274
3445.594450	456710.163546	51.106279
3444.546963	456346.996015	51.111284
3444.440948	455979.209338	51.116289
3443.307163	455615.891366	51.121293
3442.879378	455239.772502	51.126298
3442.171299	454885.456717	51.131303
3441.377958	454524.350313	51.136308
3440.780552	454147.834131	51.141313
3440.112445	453793.697817	51.146317
3439.443195	453420.428042	51.151322
3438.611845	453055.600346	51.156327
3437.687339	452693.419965	51.161332
3437.030553	452332.916669	51.166337
3436.065701	451975.602317	51.171341
3435.624215	451629.159854	51.176346
3435.166600	451267.948650	51.181351
3434.227173	450903.763336	51.186356
3433.808736	450557.199578	51.191361
3432.891233	450195.232337	51.196365
3432.299516	449842.443630	51.201370
3431.358025	449480.164520	51.206375
3430.627253	449126.219729	51.211380
3430.003172	448780.118616	51.216385
3429.222145	448424.547169	51.221389
3428.816012	448071.397767	51.226394
3428.108920	447717.021858	51.231399
3426.970917	447371.133380	51.236404
3426.279479	447006.340314	51.241409
3425.744989	446671.257765	51.246413
3425.358072	446320.007603	51.251418
3424.249162	445968.663344	51.256423
3423.320594	445622.969897	51.261428
3422.947939	445288.705024	51.266433
3422.175159	444947.291333	51.271437
3421.541499	444599.353875	51.276442
3420.871434	444258.523176	51.281447
3419.947495	443910.926136	51.286452
3419.205261	443566.899230	51.291457
3418.385323	443243.234369	51.296461
3417.669219	442907.061664	51.301466
3417.049069	442565.894508	51.306471
3416.678818	442236.256750	51.311476
3415.943907	441895.402859	51.316481
3415.053774	441557.360705	51.321485
3414.603675	441226.046668	51.326490
3413.973981	440884.197462	51.331495
3412.690859	440552.295266	51.336500
3412.273418	440214.515142	51.341505
3411.196739	439882.215869	51.346509
3410.618429	439556.763076	51.351514
3410.011901	439228.543580	51.356519
3409.226298	438907.354126	51.361524
3408.587148	438572.302665	51.366529
3408.056660	438261.675324	51.371533
3407.325601	437928.685891	51.376538
3406.683477	437596.896456	51.381543
3405.710211	437280.615076	51.386548
3405.485992	436947.938592	51.391553
3404.950473	436619.673423	51.396557
3403.592517	436292.574851	51.401562
3403.102470	435971.935531	51.406567
3402.458871	435648.117553	51.411572
3401.696126	435322.105499	51.416577
3400.764521	435008.530847	51.421581
3400.064419	434679.936394	51.426586
3399.742803	434367.145981	51.431591
3398.806140	434051.148350	51.436596
3398.074104	433724.806261	51.441601
3397.378922	433409.651147	51.446605
3396.590114	433102.327155	51.451610
3395.946961	432781.697188	51.456615
3395.097195	432473.181946	51.461620
3394.554581	432151.969637	51.466625
3393.926565	431846.992001	51.471629
3393.267774	431529.852963	51.476634
3392.742688	431221.931633	51.481639
3391.659199	430915.440732	51.486644
3391.356787	430587.518245	51.491649
3390.694794	430292.329309	51.496653
3389.911775	429978.847599	51.501658
3389.360803	429657.072520	51.506663
3388.107656	429345.333537	51.511668
3387.837441	429040.088737	51.516673
3387.191070	428728.221114	51.521677
3386.509406	428421.789877	51.526682
3386.008522	428113.294898	51.531687
3385.069952	427803.544967	51.536692
3384.489441	427491.169845	51.541697
3383.716590	427178.796070	51.546701
3382.826310	426871.770423	51.551706
3382.140735	426571.311995	51.556711
3381.546313	426271.826261	51.561716
3380.644694	425952.931530	51.566721
3379.984610	425670.135400	51.571725
3379.414568	425356.489239	51.576730
3378.686222	425054.496754	51.581735
3377.833948	424762.019452	51.586740
3377.394007	424449.129546	51.591745
3376.324755	424158.610335	51.596749
3375.972415	423857.129245	51.601754
3375.365372	423562.288939	51.606759
3374.613969	423255.454224	51.611764
3374.069268	422968.573163	51.616769
3373.186760	422669.499602	51.621773
3372.413651	422368.398848	51.626778
3371.821171	422075.546900	51.631783
3371.184385	421783.460881	51.636788
3370.689076	421481.823913	51.641793
3369.791622	421188.375757	51.646797
3369.335937	420889.291642	51.651802
3368.422732	420605.187705	51.656807
3368.033475	420297.119777	51.661812
3367.134335	420003.100546	51.666817
3366.364782	419712.487134	51.671821
3365.718577	419407.549203	51.676826
3365.222943	419118.461334	51.681831
3363.992613	418821.890946	51.686836
3363.655212	418523.143937	51.691841
3362.795338	418245.536522	51.696845
3361.906678	417944.558782	51.701850
3361.347956	417656.914010	51.706855
3360.663680	417374.316382	51.711860
3360.101210	417082.881057	51.716865
3359.436394	416803.679012	51.721869
3358.602010	416522.900492	51.726874
3358.178443	416233.390806	51.731879
3357.272195	415943.954524	51.736884
3356.540341	415653.852596	51.741889
3355.627598	415371.118924	51.746893
3354.992265	415090.269560	51.751898
3354.275917	414810.827688	51.756903
3353.591278	414532.648490	51.761908
3353.054685	414246.312733	51.766913
3352.192348	413971.942040	51.771917
3351.404214	413695.753051	51.776922
3351.069297	413414.179415	51.781927
3350.310437	413140.419782	51.786932
3349.767641	412866.039030	51.791937
3349.245631	412589.873789	51.796941
3348.588531	412299.726709	51.801946
3347.830527	412022.170549	51.806951
3347.050151	411740.600554	51.811956
3346.725739	411455.779519	51.816961
3345.573193	411185.138676	51.821965
3345.017725	410895.241322	51.826970
3344.365094	410612.903563	51.831975
3343.771964	410341.531352	51.836980
3342.799801	410063.685897	51.841985
3342.236969	409787.501140	51.846989
3341.292480	409506.927127	51.851994
3340.747736	409229.260514	51.856999
3339.889985	408965.160195	51.862004
3339.237568	408692.029073	51.867009
3338.299968	408435.814659	51.872013
3337.844098	408156.853546	51.877018
3337.246595	407892.169087	51.882023
3336.618622	407625.631975	51.887028
3336.017888	407348.160370	51.892033
3335.346443	407082.413234	51.897037
3334.736943	406810.020930	51.902042
3334.122599	406536.127541	51.907047
3333.196702	406285.001583	51.912052
3332.774569	405993.511551	51.917057
3331.938049	405732.099412	51.922061
3331.034478	405468.027081	51.927066
3330.726333	405193.412623	51.932071
3329.704176	404937.157080	51.937076
3329.215532	404655.475475	51.942081
3328.631729	404401.077833	51.947085
3327.891561	404122.633642	51.952090
3327.056743	403856.808542	51.957095
3326.157705	403599.200953	51.962100
3325.622306	403331.519496	51.967105
3325.001890	403065.018409	51.972109
3324.280755	402810.222990	51.977114
3323.862903	402551.488687	51.982119
3322.832850	402286.443817	51.987124
3322.426175	402021.526932	51.992129
3321.577712	401765.701167	51.997133
3320.748461	401495.941051	52.002138
3320.357641	401241.767193	52.007143
3319.096917	400984.449865	52.012148
3318.984657	400710.706134	52.017153
3317.955407	400464.735774	52.022157
3317.180382	400215.215468	52.027162
3316.754310	399950.030431	52.032167
3316.107865	399700.307901	52.037172
3315.514147	399435.780684	52.042177
3314.524984	399186.616819	52.047181
3314.009032	398926.216673	52.052186
3313.464818	398667.572951	52.057191
3312.806280	398424.833267	52.062196
3312.397566	398161.181664	52.067201
3311.399540	397909.696211	52.072205
3310.697738	397652.289663	52.077210
3310.018735	397397.623041	52.082215
3309.055950	397136.999805	52.087220
3308.560347	396883.088315	52.092225
3308.108141	396636.082857	52.097229
3307.405147	396375.463433	52.102234
3306.659519	396124.483868	52.107239
3305.979696	395879.313825	52.112244
3305.492264	395627.577882	52.117249
3304.979742	395369.005210	52.122253
3304.029049	395102.135582	52.127258
3303.674274	394854.110124	52.132263
3302.975044	394609.315287	52.137268
3302.122478	394344.152989	52.142273
3301.408022	394085.170261	52.147277
3300.703211	393826.743377	52.152282
3300.333341	393558.651128	52.157287
3298.986004	393309.093388	52.162292
3298.623696	393058.615316	52.167297
3297.839919	392803.625572	52.172301
3297.079380	392553.232231	52.177306
3296.654668	392303.190776	52.182311
3295.960140	392065.241907	52.187316
3295.620403	391802.063811	52.192321
3294.697799	391555.935007	52.197325
3293.886928	391295.293907	52.202330
3293.386783	391040.805745	52.207335
3292.426682	390792.770525	52.212340
3291.715304	390544.389099	52.217345
3291.356121	390294.907722	52.222349
3290.613291	390048.078809	52.227354
3290.026066	389791.637508	52.232359
3288.963512	389547.906935	52.237364
3288.396903	389289.933103	52.242369
3287.507729	389047.570197	52.247373
3287.260408	388803.603888	52.252378
3286.980045	388556.640627	52.257383
3285.579737	388311.785327	52.262388
3284.946154	388051.092322	52.267393
3284.161133	387808.882562	52.272397
3283.348603	387566.039805	52.277402
3282.938652	387332.260745	52.282407
3282.459068	387096.609434	52.287412
3281.697232	386847.091409	52.292417
3280.728071	386601.571457	52.297421
3279.954085	386361.638935	52.302426
3279.785970	386112.657726	52.307431
3278.832451	385880.099651	52.312436
3278.175535	385632.718285	52.317441
3277.461877	385396.152109	52.322445
3276.733744	385156.891074	52.327450
3276.251992	384911.308157	52.332455
3275.188312	384682.116786	52.337460
3274.759422	384435.403400	52.342465
3274.149091	384201.483498	52.347469
3273.254412	383968.904094	52.352474
3272.877535	383724.873493	52.357479
3272.005762	383492.974153	52.362484
3271.368532	383248.676447	52.367489
3271.044453	383010.558451	52.372493
3270.458974	382763.019552	52.377498
3269.636391	382522.306944	52.382503
3268.872487	382291.222411	52.387508
3268.284321	382043.984423	52.392513
3267.206276	381810.149061	52.397517
3266.602232	381573.719440	52.402522
3266.355517	381332.094365	52.407527
3265.404810	381105.559267	52.412532
3264.824335	380863.119291	52.417537
3264.242480	380632.250258	52.422541
3263.387093	380390.155985	52.427546
3262.650358	380143.870278	52.432551
3261.463348	379919.222246	52.437556
3261.088611	379673.919092	52.442561
3260.212582	379449.244591	52.447565
3259.775963	379225.084289	52.452570
3259.231903	378995.725603	52.457575
3258.458880	378776.677419	52.462580
3257.850294	378537.737361	52.467585
3257.036522	378302.134859	52.472589
3256.189781	378072.920395	52.477594
3256.039162	377833.522106	52.482599
3255.245688	377611.393001	52.487604
3254.431669	377380.617786	52.492609
3253.804360	377158.714224	52.497613
3252.933003	376926.419298	52.502618
3252.679851	376705.980194	52.507623
3251.644500	376478.414273	52.512628
3250.845539	376239.388749	52.517633
3249.947093	376015.334203	52.522637
3249.343605	375787.060151	52.527642
3248.984532	375569.251542	52.532647
3248.054795	375359.163094	52.537652
3247.535071	375119.552601	52.542657
3247.172112	374896.907955	52.547661
3245.986223	374678.385913	52.552666
3245.593409	374449.206150	52.557671
3244.816917	374229.879271	52.562676
3244.443527	374005.374475	52.567681
3243.620409	373783.457936	52.572685
3243.242302	373556.636590	52.577690
3242.386782	373331.415799	52.582695
3241.451157	373113.914260	52.587700
3240.644680	372882.603518	52.592705
3240.090283	372666.540207	52.597709
3239.463801	372450.461739	52.602714
3238.839801	372217.999143	52.607719
3238.185384	371998.793781	52.612724
3237.453474	371774.511707	52.617729
3236.849666	371558.832082	52.622733
3235.840213	371336.448639	52.627738
3235.513527	371113.218286	52.632743
3234.747177	370907.049983	52.637748
3234.656552	370685.433618	52.642753
3233.675654	370454.544147	52.647757
3232.609787	370242.543378	52.652762
3231.897941	370022.013986	52.657767
3231.263106	369807.933114	52.662772
3230.777772	369584.541772	52.667777
3230.154029	369363.766100	52.672781
3229.618537	369155.135988	52.677786
3229.030304	368932.342681	52.682791
3228.098500	368699.120902	52.687796
3227.716508	368482.703784	52.692801
3226.941973	368268.815476	52.697805
3226.152683	368046.354728	52.702810
3225.507159	367827.686326	52.707815
3224.814074	367610.372762	52.712820
3224.150162	367397.480365	52.717825
3223.438039	367175.562716	52.722829
3222.783954	366962.946529	52.727834
3222.232829	366735.760164	52.732839
3221.623061	366522.931320	52.737844
3220.776428	366302.811533	52.742849
3220.301769	366081.003504	52.747853
3219.565025	365875.595410	52.752858
3218.908371	365655.544155	52.757863
3217.908721	365429.287141	52.762868
3217.156567	365205.585022	52.767873
3216.536192	365007.609342	52.772877
3215.759398	364790.320718	52.777882
3215.481839	364565.369977	52.782887
3214.558448	364359.348423	52.787892
3213.876455	364140.489648	52.792897
3213.404982	363932.842627	52.797901
3212.860729	363713.629254	52.802906
3212.295452	363499.761381	52.807911
3211.548418	363284.776283	52.812916
3210.800735	363063.836355	52.817921
3210.090423	362860.776778	52.822925
3209.306437	362645.616443	52.827930
3208.901196	362417.825619	52.832935
3208.112440	362208.643475	52.837940
3207.101172	362000.767828	52.842945
3206.754204	361784.440269	52.847949
3205.901547	361571.728553	52.852954
3205.235785	361356.136462	52.857959
3204.491081	361156.001104	52.862964
3203.911522	360925.965991	52.867969
3203.386873	360721.315612	52.872973
3202.467586	360516.803113	52.877978
3202.010498	360301.962029	52.882983
3201.258906	360097.777445	52.887988
3200.429098	359884.596526	52.892993
3199.835965	359661.275167	52.897997
3199.351692	359469.336032	52.903002
3198.425742	359251.612666	52.908007
3197.673261	359050.706336	52.913012
3197.350888	358834.412395	52.918017
3196.424137	358620.452390	52.923021
3195.698335	358429.641543	52.928026
3195.117080	358216.770212	52.933031
3194.540728	358010.360680	52.938036
3193.694007	357804.578328	52.943041
3193.191503	357592.964181	52.948045
3191.951973	357399.126050	52.953050
3191.779574	357177.813429	52.958055
3191.064797	356982.338371	52.963060
3190.603875	356776.541605	52.968065
3189.983561	356572.397849	52.973069
3188.800960	356369.360113	52.978074
3188.473949	356155.090968	52.983079
3187.689079	355957.917986	52.988084
3186.944116	355759.618205	52.993089
3186.010942	355549.208673	52.998093
3185.599461	355346.172064	53.003098
3185.084873	355150.403720	53.008103
3184.216709	354946.292581	53.013108
3183.751572	354747.562849	53.018113
3183.089107	354540.440070	53.023117
3182.219542	354349.203761	53.028122
3181.748982	354125.252800	53.033127
3180.972020	353936.367045	53.038132
3180.327166	353736.669323	53.043137
3179.733582	353529.353436	53.048141
3179.022783	353332.387642	53.053146
3178.893616	353121.357422	53.058151
3177.840726	352925.818469	53.063156
3176.872262	352717.871521	53.068161
3176.515102	352505.169765	53.073165
3175.545276	352311.295053	53.078170
3175.243263	352107.821208	53.083175
3174.500874	351903.856347	53.088180
3173.659061	351706.014428	53.093185
3173.159549	351508.321221	53.098189
3172.348330	351306.426411	53.103194
3171.732584	351099.308057	53.108199
3170.587725	350902.478207	53.113204
3170.100287	350696.610518	53.118209
3169.818166	350504.045658	53.123213
3168.679155	350311.004853	53.128218
3168.231752	350101.921778	53.133223
3167.994476	349906.420860	53.138228
3166.811930	349694.805629	53.143233
3166.555970	349501.113228	53.148237
3165.743967	349303.003258	53.153242
3165.363463	349103.017273	53.158247
3164.263824	348903.398841	53.163252
3163.859381	348713.188529	53.168257
3163.204990	348502.223236	53.173261
3162.246827	348300.315061	53.178266
3161.667119	348087.274797	53.183271
3161.093038	347900.422708	53.188276
3160.210226	347703.641707	53.193281
3159.709029	347504.814391	53.198285
3158.689468	347308.893553	53.203290
3158.575340	347106.694830	53.208295
3157.497976	346913.810569	53.213300
3156.742221	346716.395165	53.218305
3156.509803	346517.369139	53.223309
3155.318821	346317.450513	53.228314
3154.816988	346124.039830	53.233319
3154.033101	345932.047559	53.238324
3153.322533	345738.770411	53.243329
3152.788837	345552.006007	53.248333
3152.168102	345366.501962	53.253338
3151.766094	345158.793164	53.258343
3150.762249	344972.610331	53.263348
3150.016804	344784.884287	53.268353
3149.821312	344579.787880	53.273357
3148.922484	344395.419226	53.278362
3148.599177	344187.745429	53.283367
3147.718947	343992.249424	53.288372
3147.015578	343800.746458	53.293377
3146.429343	343598.355623	53.298381
3145.235826	343400.540037	53.303386
3144.863685	343205.673761	53.308391
3143.921640	343019.958608	53.313396
3143.425732	342835.954076	53.318401
3143.076569	342638.460558	53.323405
3142.154557	342448.286003	53.328410
3141.758689	342247.744095	53.333415
3140.985897	342058.639241	53.338420
3140.078528	341862.707854	53.343425
3139.656504	341658.273614	53.348429
3138.938065	341463.812871	53.353434
3137.886304	341279.102468	53.358439
3137.316597	341092.126137	53.363444
3136.809280	340898.953850	53.368449
3136.480389	340701.069032	53.373453
3135.318056	340522.406667	53.378458
3134.569097	340333.852743	53.383463
3134.367466	340141.902490	53.388468
3133.592996	339952.893260	53.393473
3132.687435	339763.776925	53.398477
3131.916430	339582.784443	53.403482
3131.526654	339382.537739	53.408487
3130.633914	339206.196325	53.413492
3129.866023	339010.412069	53.418497
3129.466566	338815.383500	53.423501
3128.578566	338634.406823	53.428506
3128.042489	338442.606153	53.433511
3127.414566	338253.695955	53.438516
3127.096701	338065.652562	53.443521
3126.743807	337877.690532	53.448525
3125.818313	337694.884313	53.453530
3125.120435	337493.382197	53.458535
3124.292503	337306.613745	53.463540
3123.446890	337110.683282	53.468545
3123.075589	336905.207410	53.473549
3122.250938	336724.215384	53.478554
3121.537103	336529.891557	53.483559
3120.746304	336335.477509	53.488564
3120.006516	336143.269555	53.493569
3119.468312	335956.018677	53.498573
3118.413640	335779.769972	53.503578
3118.390722	335583.322978	53.508583
3117.661766	335407.530899	53.513588
3116.560788	335214.410064	53.518593
3116.332469	335030.162424	53.523597
3115.553979	334836.709459	53.528602
3114.671406	334650.196788	53.533607
3114.120648	334461.823637	53.538612
3113.307223	334269.596545	53.543617
3112.952557	334086.919253	53.548621
3112.244477	333907.937822	53.553626
3111.593219	333713.519632	53.558631
3111.269031	333529.461335	53.563636
3110.485898	333341.834711	53.568641
3109.646682	333147.724715	53.573645
3109.012599	332961.371835	53.578650
3108.536726	332766.184980	53.583655
3107.566686	332580.444323	53.588660
3106.611526	332377.847572	53.593665
3106.185715	332190.721421	53.598669
3105.381173	332016.663853	53.603674
3105.134760	331822.660092	53.608679
3104.129862	331627.961150	53.613684
3103.438328	331449.225445	53.618689
3102.874300	331265.275592	53.623693
3101.960040	331087.185236	53.628698
3101.301496	330891.283873	53.633703
3100.617904	330718.833389	53.638708
3100.040205	330531.650593	53.643713
3099.657066	330351.819588	53.648717
3098.522305	330173.558226	53.653722
3098.172043	329983.028397	53.658727
3097.523406	329797.382497	53.663732
3096.657984	329624.830930	53.668737
3096.282323	329438.733599	53.673741
3095.346725	329253.946444	53.678746
3094.769414	329065.588768	53.683751
3094.179900	328879.956697	53.688756
3093.077268	328695.983842	53.693761
3092.877749	328517.392336	53.698765
3092.298605	328353.907034	53.703770
3091.706376	328154.118148	53.708775
3091.214479	327974.502336	53.713780
3090.491172	327782.218346	53.718785
3089.603179	327595.382859	53.723789
3088.892213	327410.275636	53.728794
3088.203950	327216.635329	53.733799
3087.506044	327040.767087	53.738804
3086.800847	326851.354900	53.743809
3086.297717	326671.763315	53.748813
3085.433012	326500.146621	53.753818
3084.644274	326315.609241	53.758823
3083.946427	326122.655183	53.763828
3083.645940	325946.976223	53.768833
3082.887611	325766.837386	53.773837
3082.269497	325588.687328	53.778842
3081.654331	325394.725479	53.783847
3080.694351	325217.417970	53.788852
3079.628289	325029.942638	53.793857
3079.348491	324844.379309	53.798861
3078.952378	324676.758273	53.803866
3078.283492	324494.845673	53.808871
3077.368666	324306.555472	53.813876
3076.651539	324137.838399	53.818881
3076.226331	323953.772800	53.823885
3075.241078	323778.248446	53.828890
3074.910286	323588.616616	53.833895
3074.252721	323416.706034	53.838900
3073.620291	323235.726972	53.843905
3072.832942	323047.948445	53.848909
3071.914856	322869.076154	53.853914
3071.274997	322685.500049	53.858919
3070.842908	322514.417642	53.863924
3070.238476	322335.189065	53.868929
3069.519872	322159.950163	53.873933
3068.523248	321980.299142	53.878938
3068.129910	321796.554824	53.883943
3067.685947	321620.151065	53.888948
3066.647822	321434.038241	53.893953
3066.441770	321260.396890	53.898957
3065.226990	321087.831442	53.903962
3064.883264	320901.454839	53.908967
3064.325200	320722.648468	53.913972
3063.656761	320540.192692	53.918977
3063.327013	320355.976997	53.923981
3062.398552	320179.697962	53.928986
3061.524878	319989.151166	53.933991
3061.188417	319806.921452	53.938996
3060.389995	319634.160009	53.944001
3060.075552	319443.167104	53.949005
3059.003663	319268.589503	53.954010
3058.262224	319077.612483	53.959015
3057.861500	318900.076199	53.964020
3056.869857	318720.596094	53.969025
3056.311602	318539.621164	53.974029
3055.550871	318367.182399	53.979034
3055.013839	318171.715238	53.984039
3054.339117	317991.928961	53.989044
3053.572528	317821.450745	53.994049
3053.357020	317635.072686	53.999053
3052.438926	317448.881834	54.004058
3051.808247	317264.809475	54.009063
3051.018637	317088.884560	54.014068
3050.329040	316903.929638	54.019073
3049.595819	316718.242842	54.024077
3048.877987	316548.340306	54.029082
3048.205579	316358.798294	54.034087
3047.720118	316191.175504	54.039092
3047.132274	316003.401842	54.044097
3046.535793	315821.154700	54.049101
3045.591791	315657.906849	54.054106
3045.348132	315470.077716	54.059111
3044.467932	315290.879172	54.064116
3043.620742	315102.024477	54.069121
3043.108829	314917.139591	54.074125
3042.421313	314745.497683	54.079130
3041.509570	314561.795819	54.084135
3040.722101	314382.733785	54.089140
3040.365675	314211.318691	54.094145
3039.742080	314024.183616	54.099149
3038.990123	313859.425612	54.104154
3038.727237	313672.385607	54.109159
3037.919617	313495.515119	54.114164
3037.266715	313312.457614	54.119169
3036.471505	313133.190961	54.124173
3035.819062	312950.081833	54.129178
3035.076380	312773.199869	54.134183
3034.741394	312586.984214	54.139188
3033.953678	312412.782503	54.144193
3033.371970	312222.760204	54.149197
3032.143031	312046.310505	54.154202
3032.101389	311863.255667	54.159207
3031.429117	311682.490245	54.164212
3030.393098	311498.089783	54.169217
3029.964875	311308.168942	54.174221
3028.867439	311146.237090	54.179226
3028.366982	310954.188083	54.184231
3027.771611	310779.240367	54.189236
3027.012042	310602.179357	54.194241
3026.390832	310424.153991	54.199245
3025.834730	310255.285263	54.204250
3024.900705	310081.586908	54.209255
3024.261992	309891.646092	54.214260
3023.480240	309723.016018	54.219265
3023.221625	309539.660739	54.224269
3022.313419	309365.957235	54.229274
3021.563769	309187.160904	54.234279
3020.898273	309018.918862	54.239284
3020.095484	308851.309466	54.244289
3019.724938	308664.838384	54.249293
3019.140540	308494.138150	54.254298
3018.692065	308311.651377	54.259303
3017.760294	308148.492317	54.264308
3017.003598	307970.331925	54.269313
3016.499592	307783.116670	54.274317
3015.935612	307607.981060	54.279322
3015.182548	307436.312916	54.284327
3014.823791	307252.180618	54.289332
3013.598763	307080.179240	54.294337
3013.328840	306892.569098	54.299341
3012.532010	306717.902013	54.304346
3011.757838	306545.472047	54.309351
3011.117139	306361.179363	54.314356
3010.124503	306187.586626	54.319361
3009.858308	306011.994252	54.324365
3008.724368	305847.030722	54.329370
3008.146380	305667.336373	54.334375
3007.752518	305503.655886	54.339380
3006.662434	305320.808001	54.344385
3006.500694	305147.693571	54.349389
3005.930595	304969.932418	54.354394
3005.032194	304791.662748	54.359399
3004.621530	304618.790764	54.364404
3003.693106	304442.537177	54.369409
3003.211263	304268.479133	54.374413
3002.344961	304096.442580	54.379418
3001.852178	303919.431807	54.384423
3001.642614	303734.965441	54.389428
3000.562036	303563.013080	54.394433
2999.981905	303374.657692	54.399437
2999.163008	303202.052300	54.404442
2998.421699	303029.128832	54.409447
2997.989477	302854.297224	54.414452
2997.403586	302686.034485	54.419457
2996.898544	302506.833839	54.424461
2995.909504	302329.237541	54.429466
2995.107488	302147.485927	54.434471
2994.733858	301962.050105	54.439476
2993.672005	301801.526995	54.444481
2993.127365	301616.805401	54.449485
2992.521798	301441.210124	54.454490
2992.068944	301264.902888	54.459495
2991.375158	301091.893264	54.464500
2990.372844	300923.134216	54.469505
2989.666173	300742.562761	54.474509
2989.040757	300579.422678	54.479514
2988.702355	300394.845258	54.484519
2987.998170	300214.934937	54.489524
2986.971910	300050.991901	54.494529
2986.326779	299874.891817	54.499533
2985.754162	299711.818899	54.504538
2985.454467	299525.961042	54.509543
2984.954112	299344.158447	54.514548
2983.906366	299177.518491	54.519553
2983.622412	298997.438461	54.524557
2982.551812	298836.455366	54.529562
2981.664742	298648.855912	54.534567
2981.545039	298475.778124	54.539572
2980.658202	298299.179847	54.544577
2980.287381	298122.805318	54.549581
2979.688014	297946.746921	54.554586
2978.687490	297759.673803	54.559591
2978.257673	297586.364089	54.564596
2977.095984	297409.706562	54.569601
2976.822263	297222.976252	54.574605
2976.035529	297063.016218	54.579610
2975.312502	296884.047669	54.584615
2975.013922	296700.962528	54.589620
2974.259557	296536.718477	54.594625
2973.454776	296346.786108	54.599629
2972.650007	296187.719525	54.604634
2972.243840	295997.519981	54.609639
2971.744183	295820.425098	54.614644
2970.821355	295646.172942	54.619649
2970.392479	295454.473907	54.624653
2969.587412	295281.399743	54.629658
2968.607940	295099.108471	54.634663
2968.371900	294924.008432	54.639668
2967.264134	294739.521504	54.644673
2966.733433	294563.500044	54.649677
2966.102647	294397.350085	54.654682
2965.336762	294221.034489	54.659687
2964.735810	294048.130717	54.664692
2963.928624	293874.546366	54.669697
2963.326299	293696.803748	54.674701
2962.795729	293528.803605	54.679706
2962.178955	293350.910188	54.684711
2961.838695	293182.523116	54.689716
2961.096946	293003.706911	54.694721
2960.353611	292819.109718	54.699725
2959.406304	292642.388624	54.704730
2958.933175	292468.037211	54.709735
2958.240817	292294.433457	54.714740
2957.349338	292113.169918	54.719745
2956.959054	291930.502600	54.724749
2956.388940	291750.639564	54.729754
2955.618840	291577.658814	54.734759
2954.793687	291401.783356	54.739764
2954.040490	291227.780983	54.744769
2953.942255	291044.302749	54.749773
2953.033342	290868.083628	54.754778
2952.169830	290689.870726	54.759783
2951.836762	290513.789421	54.764788
2950.963904	290336.520059	54.769793
2950.685239	290150.472050	54.774797
2949.791436	289974.708354	54.779802
2949.233218	289800.190277	54.784807
2948.630889	289620.687399	54.789812
2948.120070	289438.623147	54.794817
2947.202052	289246.028650	54.799821
2946.379176	289076.874773	54.804826
2945.820907	288890.488161	54.809831
2945.740547	288710.188988	54.814836
2944.213503	288538.217467	54.819841
2943.799393	288342.588343	54.824845
2943.556212	288166.440404	54.829850
2942.639982	287975.602078	54.834855
2942.064562	287792.553792	54.839860
2940.842428	287617.299072	54.844865
2940.413247	287438.225891	54.849869
2939.479479	287251.948663	54.854874
2939.069703	287079.392001	54.859879
2938.786937	286897.723090	54.864884
2937.752327	286729.441900	54.869889
2937.223194	286538.668802	54.874893
2937.016480	286366.512593	54.879898
2935.730219	286171.325847	54.884903
2935.279919	285997.196047	54.889908
2934.632252	285819.098930	54.894913
2934.276282	285640.013235	54.899917
2933.629325	285453.918871	54.904922
2932.659988	285267.442492	54.909927
2932.262509	285083.855265	54.914932
2931.218120	284909.691674	54.919937
2930.688430	284712.881807	54.924941
2929.842311	284540.698654	54.929946
2929.270898	284363.021770	54.934951
2928.776356	284174.075735	54.939956
2927.790816	284005.912934	54.944961
2927.416215	283816.667611	54.949965
2926.456644	283632.481099	54.954970
2926.073575	283458.594265	54.959975
2925.773969	283272.265687	54.964980
2924.512159	283094.391983	54.969985
2924.037034	282907.556220	54.974989
2923.248040	282735.821781	54.979994
2922.668639	282552.033112	54.984999
2921.956116	282362.713382	54.990004
2921.206612	282194.156044	54.995009
2920.676885	282000.630465	55.000013
2920.052665	281828.080141	55.005018
2919.335532	281643.880017	55.010023
2918.915509	281459.887487	55.015028
2917.857561	281286.921772	55.020033
2917.234562	281099.319307	55.025037
2916.686385	280921.179142	55.030042
2915.903073	280743.432709	55.035047
2915.570719	280557.643268	55.040052
2914.798510	280379.462026	55.045057
2914.678014	280193.282398	55.050061
2913.640079	280017.766372	55.055066
2913.015522	279828.151825	55.060071
2912.748981	279630.840064	55.065076
2911.897460	279446.889861	55.070081
2910.989090	279260.274444	55.075085
2910.627927	279070.923658	55.080090
2910.028913	278895.541670	55.085095
2909.145824	278696.468126	55.090100
2908.135659	278511.702406	55.095105
2907.302844	278323.393948	55.100109
2906.662323	278146.057348	55.105114
2906.089235	277971.104075	55.110119
2905.932983	277783.070455	55.115124
2904.829408	277593.760551	55.120129
2903.906109	277412.215406	55.125133
2903.421797	277223.698816	55.130138
2902.907064	277036.562313	55.135143
2902.292365	276849.110529	55.140148
2901.773014	276664.572497	55.145153
2901.246715	276466.002471	55.150157
2900.512817	276294.792872	55.155162
2899.613632	276103.845962	55.160167
2899.150160	275915.275028	55.165172
2898.243380	275734.593062	55.170177
2897.597825	275545.439697	55.175181
2896.858008	275363.712550	55.180186
2896.309065	275184.374679	55.185191
2895.890513	274998.929218	55.190196
2895.177803	274811.416449	55.195201
2894.645267	274615.419650	55.200205
2893.739716	274432.929217	55.205210
2892.837779	274257.569366	55.210215
2892.641054	274069.185400	55.215220
2891.335836	273882.046605	55.220225
2890.751912	273697.187656	55.225229
2889.916023	273521.919250	55.230234
2889.466054	273341.292335	55.235239
2889.118669	273163.934612	55.240244
2888.193098	272978.467620	55.245249
2887.951835	272786.423340	55.250253
2887.061647	272602.147794	55.255258
2886.025772	272433.329166	55.260263
2885.821339	272250.982562	55.265268
2885.114617	272076.534289	55.270273
2884.641183	271872.302054	55.275277
2883.907040	271697.221460	55.280282
2882.973603	271515.550669	55.285287
2882.704973	271323.434504	55.290292
2881.975669	271145.449832	55.295297
2881.086857	270949.713538	55.300301
2880.592965	270758.244376	55.305306
2879.855551	270586.271611	55.310311
2879.471844	270387.806754	55.315316
2878.808985	270202.374980	55.320321
2878.121732	270011.089395	55.325325
2877.635982	269826.826674	55.330330
2876.792426	269635.616858	55.335335
2876.218904	269446.452739	55.340340
2875.435177	269252.763122	55.345345
2874.440716	269066.059763	55.350349
2874.103907	268868.351910	55.355354
2873.168827	268690.553149	55.360359
2872.531827	268506.925948	55.365364
2871.632738	268321.837667	55.370369
2871.137908	268137.525889	55.375373
2870.697441	267953.332902	55.380378
2870.208453	267766.473490	55.385383
2869.628350	267577.260020	55.390388
2868.541085	267393.984599	55.395393
2868.065441	267200.144972	55.400397
2867.508672	267017.778950	55.405402
2866.361617	266820.607557	55.410407
2865.969875	266636.916665	55.415412
2865.542261	266450.913916	55.420417
2864.745245	266266.141260	55.425421
2864.146831	266082.050340	55.430426
2863.162316	265889.870819	55.435431
2863.000053	265695.345467	55.440436
2862.071847	265517.342938	55.445441
2861.757770	265315.481505	55.450445
2860.931174	265135.272788	55.455450
2860.171107	264948.712064	55.460455
2859.495585	264749.276661	55.465460
2858.621483	264564.262252	55.470465
2858.179414	264372.506898	55.475469
2857.360542	264176.227051	55.480474
2856.485231	264001.884208	55.485479
2856.105314	263813.557477	55.490484
2855.261390	263637.630819	55.495489
2854.817951	263439.789307	55.500493
2854.267997	263257.907718	55.505498
2853.428162	263077.065370	55.510503
2852.977001	262888.419324	55.515508
2852.233801	262698.418884	55.520513
2851.647610	262507.247637	55.525517
2851.029335	262328.178833	55.530522
2850.232061	262126.955940	55.535527
2849.429283	261929.044868	55.540532
2848.713544	261750.985066	55.545537
2848.233651	261566.240917	55.550541
2847.877314	261371.825011	55.555546
2847.142332	261178.869912	55.560551
2846.743305	260988.077442	55.565556
2845.501276	260802.919611	55.570561
2844.954260	260596.513616	55.575565
2844.635401	260410.802384	55.580570
2843.476654	260220.359923	55.585575
2843.121672	260027.065283	55.590580
2842.186233	259842.012346	55.595585
2841.527029	259648.868014	55.600589
2840.913045	259461.497818	55.605594
2840.296583	259274.739370	55.610599
2839.711304	259079.138856	55.615604
2839.112963	258892.632489	55.620609
2838.327978	258701.877258	55.625613
2837.738993	258518.833275	55.630618
2837.034157	258321.851559	55.635623
2836.733915	258128.116714	55.640628
2835.895605	257940.757693	55.645633
2834.912802	257743.209237	55.650637
2834.498938	257556.088919	55.655642
2833.579395	257365.941792	55.660647
2833.097732	257173.917299	55.665652
2832.245133	256996.289844	55.670657
2831.625707	256798.990261	55.675661
2831.238858	256603.691411	55.680666
2830.543745	256416.591089	55.685671
2829.954261	256232.479341	55.690676
2829.121503	256044.968185	55.695681
2828.537176	255848.020434	55.700685
2828.174339	255647.828920	55.705690
2827.111666	255452.434376	55.710695
2826.723384	255264.369650	55.715700
2825.762052	255072.804960	55.720705
2825.360756	254872.365606	55.725709
2824.841855	254687.098008	55.730714
2823.956286	254490.912319	55.735719
2823.567694	254288.230427	55.740724
2822.760120	254097.253526	55.745729
2821.957080	253905.079142	55.750733
2821.318797	253701.826184	55.755738
2820.547701	253514.765996	55.760743
2820.016353	253323.847986	55.765748
2818.907265	253129.660017	55.770753
2818.441982	252936.210714	55.775757
2818.102042	252756.774008	55.780762
2817.197550	252569.201080	55.785767
2817.044943	252367.757207	55.790772
2816.089352	252181.466110	55.795777
2815.195211	251976.345541	55.800781
2814.658964	251784.080169	55.805786
2813.780251	251588.329363	55.810791
2813.113719	251391.450110	55.815796
2812.329429	251207.475849	55.820801
2812.093720	251020.562657	55.825805
2811.695185	250820.432825	55.830810
2810.730285	250629.433540	55.835815
2809.865753	250436.788721	55.840820
2809.325090	250243.074180	55.845825
2808.527214	250055.181484	55.850829
2808.049104	249869.912345	55.855834
2807.016496	249680.223665	55.860839
2806.577345	249481.247869	55.865844
2805.916340	249297.459929	55.870849
2805.507160	249104.056987	55.875853
2805.049161	248915.398741	55.880858
2803.895125	248727.232934	55.885863
2803.459196	248517.103615	55.890868
2802.725663	248324.924443	55.895873
2802.241807	248129.522703	55.900877
2801.681052	247934.846442	55.905882
2800.732195	247744.841252	55.910887
2800.176447	247548.254739	55.915892
2799.491414	247363.174139	55.920897
2798.716086	247168.914841	55.925901
2798.042213	246963.791232	55.930906
2797.058511	246782.578551	55.935911
2796.779807	246587.248212	55.940916
2796.116671	246394.194543	55.945921
2795.616725	246203.712807	55.950925
2794.624751	246016.186877	55.955930
2793.988488	245830.260141	55.960935
2793.410922	245623.366061	55.965940
2792.608660	245439.146869	55.970945
2792.321458	245242.240858	55.975949
2792.013080	245040.296289	55.980954
2790.862647	244853.790178	55.985959
2790.070443	244653.730855	55.990964
2789.422791	244459.302280	55.995969
2788.418650	244261.976445	56.000973
2788.111163	244073.173364	56.005978
2787.398006	243893.067564	56.010983
2786.917137	243691.992695	56.015988
2785.980731	243505.963885	56.020993
2785.567644	243316.720237	56.025997
2784.837061	243114.590798	56.031002
2784.042385	242934.702956	56.036007
2783.680138	242730.733226	56.041012
2782.879269	242547.027136	56.046017
2782.113003	242359.979906	56.051021
2781.355985	242167.736618	56.056026
2780.911912	241977.022898	56.061031
2780.131110	241774.266931	56.066036
2779.373871	241593.076369	56.071041
2778.793604	241406.128447	56.076045
2778.474091	241206.025112	56.081050
2777.487205	241017.308711	56.086055
2776.687598	240824.208469	56.091060
2776.268716	240634.995280	56.096065
2775.901996	240435.333604	56.101069
2775.159923	240240.646385	56.106074
2774.400368	240051.691794	56.111079
2773.868645	239850.376574	56.116084
2773.007382	239663.908780	56.121089
2772.196354	239462.994967	56.126093
2771.945061	239274.699618	56.131098
2771.152117	239073.452584	56.136103
2770.745614	238882.508698	56.141108
2770.088205	238669.068954	56.146113
2769.349059	238478.815036	56.151117
2768.444901	238273.716470	56.156122
2767.728827	238085.012886	56.161127
2767.423667	237876.433455	56.166132
2766.636008	237681.070296	56.171137
2766.021491	237487.615331	56.176141
2765.344657	237282.890030	56.181146
2764.805295	237091.333666	56.186151
2764.263305	236879.228692	56.191156
2763.506757	236684.575388	56.196161
2762.830198	236480.717338	56.201165
2762.065038	236273.334249	56.206170
2761.533922	236074.342987	56.211175
2761.072428	235866.123232	56.216180
2760.290245	235677.001454	56.221185
2759.131341	235470.471682	56.226189
2758.616851	235262.668943	56.231194
2757.621213	235076.153882	56.236199
2757.335278	234874.987156	56.241204
2756.654948	234684.450582	56.246209
2755.927664	234479.509567	56.251213
2755.185652	234293.745135	56.256218
2754.509341	234092.107059	56.261223
2753.839736	233891.639633	56.266228
2753.226881	233692.003904	56.271233
2752.450637	233502.146806	56.276237
2752.309475	233301.826048	56.281242
2751.310799	233115.595207	56.286247
2750.385526	232903.711948	56.291252
2749.808848	232714.715971	56.296257
2749.145097	232516.745784	56.301261
2748.595749	232314.658382	56.306266
2747.800627	232130.179592	56.311271
2747.293735	231930.454308	56.316276
2746.447796	231738.065443	56.321281
2745.839916	231557.377499	56.326285
2745.413643	231351.886132	56.331290
2744.652701	231155.283684	56.336295
2744.186209	230949.723182	56.341300
2743.324544	230768.618632	56.346305
2742.502274	230573.122009	56.351309
2741.822291	230370.881239	56.356314
2740.915784	230177.232080	56.361319
2740.681342	229983.044034	56.366324
2740.237672	229785.706783	56.371329
2739.250913	229598.564392	56.376333
2738.771660	229394.766280	56.381338
2737.756802	229198.641104	56.386343
2737.333443	229002.626372	56.391348
2736.415811	228813.310418	56.396353
2736.069150	228614.941909	56.401357
2735.318131	228422.901459	56.406362
2734.249534	228228.365567	56.411367
2734.148106	228026.394920	56.416372
2733.503051	227840.500662	56.421377
2732.351288	227652.497372	56.426381
2732.335582	227457.134448	56.431386
2731.231135	227257.208597	56.436391
2730.507480	227052.690797	56.441396
2729.871964	226864.327394	56.446401
2729.251105	226670.742550	56.451405
2728.927550	226474.514029	56.456410
2727.913592	226286.593767	56.461415
2727.611224	226085.945306	56.466420
2726.799674	225890.737495	56.471425
2726.230096	225704.390387	56.476429
2725.825300	225495.421138	56.481434
2724.969883	225298.146615	56.486439
2724.333336	225093.785291	56.491444
2723.658199	224888.781344	56.496449
2722.654381	224703.179986	56.501453
2722.281205	224495.379462	56.506458
2721.463675	224301.118414	56.511463
2720.675261	224091.678847	56.516468
2720.205498	223898.165690	56.521473
2719.469086	223709.316267	56.526477
2718.901124	223520.580642	56.531482
2718.447816	223312.210288	56.536487
2717.847421	223110.992592	56.541492
2717.046985	222912.263981	56.546497
2716.294167	222709.314716	56.551501
2715.801988	222498.228462	56.556506
2714.889259	222310.556010	56.561511
2714.077563	222118.858103	56.566516
2713.324955	221913.734074	56.571521
2712.846911	221718.356313	56.576525
2712.291325	221523.500522	56.581530
2711.634784	221336.973731	56.586535
2711.024924	221136.322767	56.591540
2710.311007	220940.526087	56.596545
2709.422877	220743.319059	56.601549
2709.211497	220535.707111	56.606554
2708.138608	220346.791896	56.611559
2707.413604	220146.441854	56.616564
2707.270617	219947.145818	56.621569
2706.455621	219747.956757	56.626573
2705.700075	219554.283388	56.631578
2704.991720	219353.258193	56.636583
2704.532410	219149.049947	56.641588
2704.125705	218949.403766	56.646593
2703.173076	218753.790681	56.651597
2702.494393	218553.106676	56.656602
2701.773962	218364.751725	56.661607
2701.049652	218161.530189	56.666612
2700.249975	217950.518196	56.671617
2699.594358	217767.106182	56.676621
2699.314912	217560.799083	56.681626
2698.376993	217366.854950	56.686631
2697.918914	217150.139521	56.691636
2697.319662	216964.976775	56.696641
2696.168507	216764.028951	56.701645
2695.853660	216562.961962	56.706650
2695.000644	216357.372947	56.711655
2694.410279	216161.913265	56.716660
2693.847170	215976.721951	56.721665
2692.882449	215777.554928	56.726669
2692.418212	215577.125432	56.731674
2691.689106	215380.009746	56.736679
2691.179640	215183.356253	56.741684
2690.486947	214991.441934	56.746689
2689.662345	214792.535606	56.751693
2689.316919	214582.505590	56.756698
2688.356049	214390.139038	56.761703
2687.786370	214193.574319	56.766708
2686.981083	213985.553730	56.771713
2686.204088	213794.407141	56.776717
2685.697405	213597.350513	56.781722
2684.776552	213410.415439	56.786727
2684.287887	213201.787095	56.791732
2683.780710	213013.667524	56.796737
2682.938937	212819.479228	56.801741
2682.367543	212621.786617	56.806746
2681.599541	212432.780868	56.811751
2680.979532	212228.911277	56.816756
2680.553911	212045.503684	56.821761
2679.970578	211847.688028	56.826765
2679.489887	211643.989125	56.831770
2678.725374	211449.729034	56.836775
2677.990809	211245.307930	56.841780
2677.221145	211039.378424	56.846785
2676.371401	210844.140897	56.851789
2676.208297	210645.880541	56.856794
2675.458460	210447.650107	56.861799
2674.972416	210249.582150	56.866804
2674.277312	210043.249503	56.871809
2673.579094	209839.756283	56.876813
2673.052405	209634.760153	56.881818
2672.008977	209432.532058	56.886823
2671.507053	209228.373356	56.891828
2670.846085	209021.275024	56.896833
2669.965883	208822.599469	56.901837
2669.398943	208623.925839	56.906842
2668.639648	208422.496039	56.911847
2667.655501	208224.806155	56.916852
2667.265998	208019.450008	56.921857
2666.565680	207830.523684	56.926861
2666.212441	207628.064911	56.931866
2664.999875	207430.121066	56.936871
2664.708464	207235.200987	56.941876
2664.127788	207034.752923	56.946881
2663.297237	206843.279454	56.951885
2662.773769	206628.454919	56.956890
2662.386799	206437.523371	56.961895
2661.875408	206233.325305	56.966900
2660.575830	206027.738310	56.971905
2660.248888	205837.015538	56.976909
2659.531331	205634.048513	56.981914
2658.497969	205434.988400	56.986919
2657.950551	205231.346752	56.991924
2657.397670	205028.444819	56.996929
2656.504305	204824.732123	57.001933
2655.951853	204631.249152	57.006938
2655.107925	204440.651002	57.011943
2654.727621	204237.151799	57.016948
2654.247462	204049.806180	57.021953
2653.442601	203853.464182	57.026957
2652.661786	203641.440254	57.031962
2652.125944	203453.621802	57.036967
2651.477436	203249.201391	57.041972
2650.554117	203051.977350	57.046977
2649.743856	202859.457473	57.051981
2649.485798	202653.679288	57.056986
2648.654884	202464.180106	57.061991
2648.062385	202256.012955	57.066996
2647.625552	202052.097829	57.072001
2646.805905	201861.262674	57.077005
2646.451000	201671.499873	57.082010
2645.501943	201473.738233	57.087015
2645.277992	201266.585349	57.092020
2644.810016	201065.249369	57.097025
2643.654329	200853.753462	57.102029
2642.867024	200651.044308	57.107034
2642.409277	200448.054632	57.112039
2641.575906	200250.419031	57.117044
2641.232210	200052.502962	57.122049
2640.243467	199841.404456	57.127053
2639.867613	199640.682659	57.132058
2639.391900	199443.565968	57.137063
2638.551019	199235.347774	57.142068
2638.090104	199030.276946	57.147073
2637.214477	198830.095446	57.152077
2636.952431	198615.336281	57.157082
2635.959307	198417.847215	57.162087
2635.390155	198200.186151	57.167092
2634.584250	197985.528407	57.172097
2633.652324	197788.362834	57.177101
2633.273052	197575.891474	57.182106
2632.351546	197383.064949	57.187111
2631.927407	197175.106906	57.192116
2631.246317	196969.340875	57.197121
2630.420313	196766.957930	57.202125
2629.795489	196560.166621	57.207130
2628.863257	196370.437613	57.212135
2628.644614	196150.286384	57.217140
2627.736038	195951.126280	57.222145
2627.100809	195751.325589	57.227149
2626.304404	195542.478717	57.232154
2625.533705	195348.108920	57.237159
2624.750259	195148.550367	57.242164
2624.576633	194948.819634	57.247169
2623.647757	194755.329674	57.252173
2623.207823	194551.252843	57.257178
2622.610495	194355.027085	57.262183
2621.961853	194141.034730	57.267188
2621.504827	193940.245871	57.272193
2620.343352	193732.227706	57.277197
2620.018114	193519.662728	57.282202
2619.263514	193328.619058	57.287207
2618.653114	193131.496749	57.292212
2618.041492	192915.493395	57.297217
2616.973875	192718.648738	57.302221
2616.468568	192509.984589	57.307226
2615.937806	192313.501813	57.312231
2615.189350	192109.420193	57.317236
2614.615180	191905.197296	57.322241
2613.912127	191695.804512	57.327245
2613.419148	191491.735876	57.332250
2612.621532	191301.215789	57.337255
2611.581277	191088.125655	57.342260
2611.580430	190894.338278	57.347265
2610.631447	190690.637877	57.352269
2610.010817	190485.843016	57.357274
2609.017998	190285.115750	57.362279
2608.861291	190075.516155	57.367284
2607.832647	189865.623039	57.372289
2607.301696	189672.637038	57.377293
2606.814905	189461.756517	57.382298
2605.828771	189257.228370	57.387303
2605.128575	189064.958670	57.392308
2604.765615	188860.626117	57.397313
2603.988085	188656.105675	57.402317
2603.390419	188449.878244	57.407322
2602.664395	188240.847655	57.412327
2602.140283	188041.938516	57.417332
2601.462943	187836.438853	57.422337
2600.563308	187634.753845	57.427341
2600.129893	187420.960564	57.432346
2599.446401	187224.802718	57.437351
2598.648109	187018.498875	57.442356
2598.391682	186815.519622	57.447361
2597.311531	186618.473029	57.452365
2596.675095	186404.449433	57.457370
2596.054026	186205.474455	57.462375
2595.427814	185996.705299	57.467380
2594.995883	185797.663954	57.472385
2594.011569	185594.309261	57.477389
2593.370519	185376.627321	57.482394
2592.614644	185185.285724	57.487399
2592.054303	184976.638011	57.492404
2591.555526	184774.609429	57.497409
2590.878773	184574.607222	57.502413
2590.074170	184366.026470	57.507418
2589.407822	184171.634553	57.512423
2588.682050	183967.393870	57.517428
2588.140258	183750.149283	57.522433
2587.563684	183553.570487	57.527437
2586.993820	183348.086693	57.532442
2586.258205	183152.501671	57.537447
2585.882106	182941.175519	57.542452
2585.091822	182739.227747	57.547457
2583.944652	182523.929609	57.552461
2583.662327	182325.706794	57.557466
2583.029325	182115.404801	57.562471
2582.244754	181908.600589	57.567476
2581.821191	181700.111906	57.572481
2580.662882	181506.140365	57.577485
2580.225828	181292.974578	57.582490
2579.631283	181094.794082	57.587495
2578.650876	180885.100038	57.592500
2578.177728	180678.265038	57.597505
2577.365790	180478.429996	57.602509
2576.857054	180263.334420	57.607514
2576.092953	180073.326428	57.612519
2575.382200	179866.571129	57.617524
2574.998765	179668.312850	57.622529
2574.078730	179463.945868	57.627533
2573.471663	179263.435299	57.632538
2573.033529	179055.724888	57.637543
2572.350756	178861.257436	57.642548
2571.796193	178649.051922	57.647553
2570.856274	178446.588226	57.652557
2570.503621	178238.779234	57.657562
2569.484374	178037.805548	57.662567
2569.079484	177831.889337	57.667572
2568.720331	177622.634392	57.672577
2567.756574	177418.640366	57.677581
2567.044444	177209.659645	57.682586
2566.379414	177002.186101	57.687591
2565.601727	176800.213419	57.692596
2565.041825	176596.782665	57.697601
2564.362501	176391.514847	57.702605
2563.767388	176183.029512	57.707610
2563.097114	175974.111975	57.712615
2562.343348	175779.899045	57.717620
2561.959462	175566.702806	57.722625
2561.237500	175362.629721	57.727629
2560.479266	175151.339180	57.732634
2559.709893	174951.282050	57.737639
2558.798832	174745.448686	57.742644
2558.796027	174536.496311	57.747649
2557.653156	174331.426730	57.752653
2557.155469	174122.987331	57.757658
2556.433872	173925.318740	57.762663
2555.636359	173722.092555	57.767668
2555.577519	173510.114698	57.772673
2554.711920	173302.030359	57.777677
2553.595159	173091.379700	57.782682
2552.841385	172885.976030	57.787687
2552.312205	172686.349916	57.792692
2552.044703	172482.155779	57.797697
2550.819738	172284.129926	57.802701
2550.412042	172070.027527	57.807706
2549.840910	171875.575528	57.812711
2549.022511	171674.550518	57.817716
2548.535985	171468.107144	57.822721
2547.677809	171254.512944	57.827725
2547.006879	171052.399474	57.832730
2546.531017	170846.771585	57.837735
2545.375845	170649.226147	57.842740
2545.255344	170440.263029	57.847745
2544.272901	170250.449729	57.852749
2543.755176	170042.327435	57.857754
2543.404124	169841.047024	57.862759
2542.351020	169645.906735	57.867764
2542.176989	169425.741217	57.872769
2541.143295	169227.586068	57.877773
2540.936660	169010.352948	57.882778
2540.079923	168809.743013	57.887783
2539.492306	168608.328484	57.892788
2538.946911	168390.046211	57.897793
2538.126735	168188.073069	57.902797
2537.155957	167966.236438	57.907802
2536.613013	167764.984588	57.912807
2535.881270	167561.551095	57.917812
2535.568416	167358.332068	57.922817
2534.976136	167147.694055	57.927821
2533.737170	166931.602789	57.932826
2533.340124	166732.876509	57.937831
2532.488298	166528.056135	57.942836
2532.019872	166311.897183	57.947841
2531.221715	166114.318582	57.952845
2530.649295	165897.491849	57.957850
2530.042089	165707.628989	57.962855
2529.276385	165498.579015	57.967860
2528.711818	165290.591871	57.972865
2527.694621	165087.725637	57.977869
2527.613756	164881.558727	57.982874
2526.677211	164681.466595	57.987879
2526.060501	164488.458090	57.992884
2525.951437	164196.293946	57.997889
2524.826997	163996.464181	58.002893
2524.063604	163786.482609	58.007898
2523.498188	163571.664639	58.012903
2522.655111	163372.543867	58.017908
2522.062990	163161.152827	58.022913
2520.995675	162962.107977	58.027917
2520.576969	162751.073276	58.032922
2520.203387	162552.670890	58.037927
2519.554904	162346.328475	58.042932
2518.949306	162131.525376	58.047937
2517.831432	161933.155339	58.052941
2517.359871	161716.833178	58.057946
2516.792926	161511.296328	58.062951
2516.064696	161325.353203	58.067956
2515.699775	161103.182068	58.072961
2514.851297	160901.037120	58.077965
2514.094561	160682.961011	58.082970
2513.349515	160496.783298	58.087975
2512.716950	160290.246762	58.092980
2512.072116	160074.050996	58.097985
2511.314806	159883.873640	58.102989
2510.946769	159655.151827	58.107994
2510.048823	159463.346266	58.112999
2509.371183	159264.234791	58.118004
2509.309269	159050.749844	58.123009
2508.015690	158845.635978	58.128013
2507.768046	158634.801914	58.133018
2507.150094	158430.664020	58.138023
2506.108614	158221.572812	58.143028
2505.713112	158013.778901	58.148033
2504.695332	157807.724805	58.153037
2504.219822	157596.856846	58.158042
2503.413084	157388.737749	58.163047
2502.827790	157197.937512	58.168052
2502.523339	156996.605977	58.173057
2501.591135	156782.103299	58.178061
2500.908933	156565.502931	58.183066
2500.152685	156365.047567	58.188071
2499.291634	156159.537806	58.193076
2498.856994	155947.681897	58.198081
2498.001697	155754.186635	58.203085
2497.540103	155554.299498	58.208090
2496.810517	155351.150904	58.213095
2496.031927	155141.274011	58.218100
2495.790885	154941.838565	58.223105
2494.969869	154730.966701	58.228109
2494.174924	154507.596507	58.233114
2493.509326	154319.901266	58.238119
2492.795901	154117.418505	58.243124
2492.414954	153905.236328	58.248129
2491.424435	153713.935081	58.253133
2490.816203	153505.261638	58.258138
2490.183784	153298.716090	58.263143
2489.343096	153103.276170	58.268148
2488.871942	152894.711919	58.273153
2488.147796	152694.082549	58.278157
2487.291868	152492.255033	58.283162
2486.736067	152293.317363	58.288167
2486.120178	152092.521937	58.293172
2485.778923	151883.015563	58.298177
2485.013231	151685.106238	58.303181
2484.188168	151492.418796	58.308186
2483.674530	151270.423828	58.313191
2482.861692	151067.390693	58.318196
2482.161836	150864.544269	58.323201
2481.378138	150668.219980	58.328205
2480.821797	150461.362321	58.333210
2480.172603	150265.260623	58.338215
2479.648192	150070.919713	58.343220
2479.203423	149864.505709	58.348225
2478.344852	149668.046784	58.353229
2477.718004	149459.452713	58.358234
2477.076489	149260.534306	58.363239
2476.310807	149051.405643	58.368244
2475.552869	148836.202000	58.373249
2474.951514	148649.265980	58.378253
2474.535332	148436.603545	58.383258
2473.557650	148222.328479	58.388263
2472.812231	148024.590701	58.393268
2472.582114	147820.634009	58.398273
2471.622635	147619.602894	58.403277
2471.211266	147405.319788	58.408282
2470.570973	147205.867422	58.413287
2469.559656	147004.950067	58.418292
2469.004061	146800.200000	58.423297
2468.267306	146590.638015	58.428301
2467.693096	146382.093744	58.433306
2466.907785	146178.959947	58.438311
2466.436188	145981.903127	58.443316
2465.768629	145766.693154	58.448321
2464.931704	145577.766474	58.453325
2464.257696	145376.107060	58.458330
2463.610597	145170.085845	58.463335
2462.976141	144964.368968	58.468340
2462.308214	144769.206220	58.473345
2461.442081	144568.090772	58.478349
2460.967396	144363.826619	58.483354
2460.526589	144169.114516	58.488359
2459.479545	143969.124459	58.493364
2459.162208	143756.795522	58.498369
2458.392318	143564.909577	58.503373
2457.649173	143363.261431	58.508378
2457.201247	143163.041837	58.513383
2456.326626	142955.394008	58.518388
2455.851733	142748.344984	58.523393
2455.017956	142560.414571	58.528397
2454.409950	142354.240661	58.533402
2454.138669	142149.348969	58.538407
2453.105947	141939.674577	58.543412
2452.519896	141730.375553	58.548417
2451.758719	141536.658437	58.553421
2451.094562	141340.284244	58.558426
2450.610301	141129.270556	58.563431
2449.855679	140929.406417	58.568436
2449.127657	140705.562916	58.573441
2448.261101	140524.702140	58.578445
2447.652498	140313.218303	58.583450
2447.091467	140118.144392	58.588455
2446.479636	139920.348049	58.593460
2445.944309	139715.832265	58.598465
2445.396866	139520.264550	58.603469
2444.494632	139320.713984	58.608474
2443.828329	139118.878484	58.613479
2443.316650	138914.948860	58.618484
2442.647864	138698.060737	58.623489
2442.064571	138499.735621	58.628493
2441.215684	138302.228935	58.633498
2440.851799	138095.270377	58.638503
2439.805064	137891.330929	58.643508
2439.434812	137680.221762	58.648513
2438.583058	137475.796892	58.653517
2437.747436	137274.547045	58.658522
2437.426177	137083.342587	58.663527
2436.548846	136875.025624	58.668532
2436.180982	136667.849001	58.673537
2435.142449	136465.353700	58.678541
2434.649751	136267.245163	58.683546
2434.235773	136062.811527	58.688551
2433.243522	135864.886531	58.693556
2432.499934	135646.609817	58.698561
2432.146155	135450.746094	58.703565
2431.504067	135249.987613	58.708570
2430.673860	135047.519930	58.713575
2430.213019	134843.216602	58.718580
2429.708450	134636.152276	58.723585
2428.951926	134429.358031	58.728589
2428.073216	134224.490133	58.733594
2427.782058	134012.200777	58.738599
2426.652509	133818.478163	58.743604
2426.139666	133594.489306	58.748609
2425.664250	133391.595890	58.753613
2424.982337	133181.597622	58.758618
2424.168475	132980.793221	58.763623
2423.510095	132785.973961	58.768628
2422.937086	132566.588345	58.773633
2422.431375	132363.821337	58.778637
2421.284598	132160.522271	58.783642
2421.067814	131947.258332	58.788647
2419.998751	131754.848449	58.793652
2419.435285	131544.246452	58.798657
2419.129951	131344.071597	58.803661
2418.209135	131126.581326	58.808666
2417.398816	130935.545914	58.813671
2416.958482	130725.362359	58.818676
2416.600330	130513.630439	58.823681
2415.442205	130308.796874	58.828685
2414.999920	130100.955385	58.833690
2414.562261	129891.755652	58.838695
2413.492658	129690.850004	58.843700
2413.025221	129476.590269	58.848705
2412.225781	129272.266280	58.853709
2411.621115	129055.148377	58.858714
2411.218692	128852.809392	58.863719
2410.431266	128640.969178	58.868724
2409.825207	128435.388697	58.873729
2409.094845	128232.458478	58.878733
2408.123968	128031.980981	58.883738
2407.913570	127819.763459	58.888743
2406.704738	127617.243817	58.893748
2406.386192	127405.160930	58.898753
2405.571644	127206.239484	58.903757
2405.153553	126989.413014	58.908762
2404.343990	126793.617985	58.913767
2403.427056	126590.513536	58.918772
2403.072192	126372.627828	58.923777
2402.491425	126172.076651	58.928781
2401.850271	125964.539038	58.933786
2401.407689	125754.736413	58.938791
2400.348591	125551.281248	58.943796
2399.820740	125340.834962	58.948801
2399.210298	125126.936515	58.953805
2398.795867	124917.783548	58.958810
2398.363456	124699.491756	58.963815
2397.542150	124496.476675	58.968820
2396.848043	124283.283902	58.973825
2396.141674	124077.383822	58.978829
2395.271083	123867.523985	58.983834
2395.146627	123647.464877	58.988839
2393.953743	123448.592831	58.993844
2393.410733	123224.159101	58.998849
2392.555908	123015.535167	59.003853
2392.023225	122806.201490	59.008858
2391.707362	122587.629020	59.013863
2390.507495	122383.712199	59.018868
2390.185459	122166.972659	59.023873
2389.485041	121953.380414	59.028877
2388.691047	121736.058929	59.033882
2387.914543	121527.370757	59.038887
2387.131634	121320.869200	59.043892
2386.696728	121109.577990	59.048897
2386.045657	120899.655947	59.053901
2385.481670	120679.475209	59.058906
2384.961389	120463.327028	59.063911
2384.139673	120269.244829	59.068916
2383.719300	120050.379766	59.073921
2382.849959	119833.136705	59.078925
2381.984622	119614.853692	59.083930
2381.561651	119408.094258	59.088935
2380.799362	119201.155372	59.093940
2380.344664	118987.910099	59.098945
2379.581568	118770.290848	59.103949
2379.000100	118555.329843	59.108954
2378.206537	118336.220923	59.113959
2377.273437	118131.609254	59.118964
2376.751984	117907.268217	59.123969
2376.116248	117707.449841	59.128973
2375.382279	117489.646297	59.133978
2375.061295	117285.826623	59.138983
2374.166936	117062.694640	59.143988
2373.590233	116853.104473	59.148993
2372.886482	116641.600153	59.153997
2372.307492	116426.078866	59.159002
2371.740429	116211.934900	59.164007
2370.793553	116008.211908	59.169012
2370.275672	115781.648228	59.174017
2369.657808	115571.745020	59.179021
2368.722917	115361.804942	59.184026
2368.021081	115156.228255	59.189031
2367.300215	114948.136434	59.194036
2366.978680	114733.280482	59.199041
2366.353507	114524.447052	59.204045
2365.668480	114305.342724	59.209050
2365.056396	114086.723792	59.214055
2364.082188	113877.468682	59.219060
2363.564242	113668.618984	59.224065
2362.815677	113461.153098	59.229069
2362.298508	113249.253964	59.234074
2361.629744	113030.634154	59.239079
2360.837958	112819.067795	59.244084
2360.169769	112610.879034	59.249089
2359.557552	112397.529775	59.254093
2359.186822	112182.633599	59.259098
2358.498460	111966.774212	59.264103
2357.498295	111766.210032	59.269108
2356.980780	111539.202140	59.274113
2356.284899	111327.233422	59.279117
2355.829598	111114.454140	59.284122
2355.270286	110896.235517	59.289127
2354.762253	110695.011788	59.294132
2353.769301	110466.642204	59.299137
2353.101141	110248.446562	59.304141
2352.659702	110034.754220	59.309146
2351.763630	109816.389129	59.314151
2351.084364	109613.786260	59.319156
2350.628635	109385.392305	59.324161
2350.018983	109176.398213	59.329165
2349.212746	108957.391964	59.334170
2348.939971	108738.988416	59.339175
2348.031751	108529.044601	59.344180
2347.488577	108303.371461	59.349185
2346.669449	108074.457257	59.354189
2345.625217	107872.485096	59.359194
2344.934229	107643.186611	59.364199
2344.239979	107435.140939	59.369204
2343.805197	107223.965821	59.374209
2342.971377	107011.085531	59.379213
2342.396110	106801.478240	59.384218
2341.901128	106582.463103	59.389223
2340.934064	106377.750160	59.394228
2340.422392	106154.566591	59.399233
2339.734378	105955.301325	59.404237
2338.853478	105736.056881	59.409242
2338.681265	105517.070069	59.414247
2337.773733	105310.605654	59.419252
2337.513791	105096.014421	59.424257
2336.950701	104879.290659	59.429261
2335.638798	104657.313817	59.434266
2335.271006	104439.370328	59.439271
2334.503433	104231.548050	59.444276
2334.112654	104010.198869	59.449281
2333.074465	103796.117068	59.454285
2332.492102	103582.301170	59.459290
2332.299621	103365.208907	59.464295
2331.709241	103152.889035	59.469300
2330.765681	102929.004823	59.474305
2330.295155	102711.271161	59.479309
2329.566713	102489.983415	59.484314
2329.185747	102278.875280	59.489319
2327.624703	102051.474996	59.494324
2327.303641	101839.891871	59.499329
2326.953963	101624.648554	59.504333
2326.349455	101402.437933	59.509338
2325.964791	101178.773613	59.514343
2324.985934	100966.446316	59.519348
2324.404758	100743.381903	59.524353
2323.591672	100518.129878	59.529357
2323.015532	100296.851437	59.534362
2322.417739	100082.682978	59.539367
2321.540651	99862.274682	59.544372
2320.919462	99633.416922	59.549377
2320.353773	99412.627349	59.554381
2319.710516	99191.516007	59.559386
2319.251923	98973.339660	59.564391
2318.542740	98749.946863	59.569396
2317.657183	98522.359884	59.574401
2317.190811	98299.059825	59.579405
2316.486841	98072.177934	59.584410
2316.091611	97849.543297	59.589415
2315.119305	97619.904993	59.594420
2314.793934	97393.610398	59.599425
2314.007293	97167.898583	59.604429
2313.306433	96943.234580	59.609434
2312.382849	96710.020611	59.614439
2311.917652	96495.636273	59.619444
2311.221340	96264.731131	59.624449
2310.456808	96036.902408	59.629453
2310.006634	95822.338131	59.634458
2309.239963	95588.362456	59.639463
2308.337575	95373.233608	59.644468
2308.072894	95142.778834	59.649473
2307.409601	94917.672356	59.654477
2306.614536	94708.570247	59.659482
2306.191317	94473.251632	59.664487
2305.303414	94245.619119	59.669492
2304.521185	94018.346313	59.674497
2303.930608	93784.640513	59.679501
2303.113499	93562.596921	59.684506
2302.699150	93337.054649	59.689511
2302.218092	93122.958610	59.694516
2301.266635	92882.610381	59.699521
2300.329656	92662.960044	59.704525
2299.601959	92444.629351	59.709530
2298.949142	92204.361586	59.714535
2298.089346	92005.688049	59.719540
2297.452962	91782.530249	59.724545
2296.818742	91566.755122	59.729549
2296.508926	91352.725107	59.734554
2296.069009	91124.603317	59.739559
2295.229195	90914.491407	59.744564
2294.979733	90674.208031	59.749569
2294.361649	90450.306285	59.754573
2293.262438	90231.498436	59.759578
2292.618073	89998.544929	59.764583
2291.978663	89773.131784	59.769588
2291.090257	89565.874637	59.774593
2290.435108	89329.227245	59.779597
2289.635075	89106.541046	59.784602
2289.095221	88884.487914	59.789607
2288.538688	88671.417168	59.794612
2288.037212	88443.244332	59.799617
2287.245546	88223.577331	59.804621
2286.400190	88000.662398	59.809626
2285.852470	87771.755863	59.814631
2285.117488	87557.101389	59.819636
2284.925365	87328.384067	59.824641
2284.165452	87108.900864	59.829645
2283.449696	86892.709437	59.834650
2282.699017	86658.623147	59.839655
2281.874740	86433.907985	59.844660
2281.454407	86209.435405	59.849665
2281.078148	85988.375032	59.854669
2279.906083	85764.850421	59.859674
2279.432992	85535.727637	59.864679
2278.320201	85316.420161	59.869684
2278.110612	85088.502841	59.874689
2277.595189	84875.906878	59.879693
2276.805536	84646.419143	59.884698
2276.371120	84419.508140	59.889703
2275.622362	84188.858867	59.894708
2275.049724	83967.096292	59.899713
2274.261943	83733.548728	59.904718
2273.270731	83512.465799	59.909722
2272.877186	83275.666169	59.914727
2272.084620	83056.914402	59.919732
2271.444380	82832.962361	59.924737
2270.817267	82612.312837	59.929742
2270.314147	82388.654351	59.934746
2269.861005	82151.940188	59.939751
2268.703322	81925.608020	59.944756
2268.131685	81710.536636	59.949761
2267.765215	81477.238845	59.954766
2266.728893	81261.935210	59.959770
2266.271307	81020.703002	59.964775
2265.516255	80807.222752	59.969780
2265.024698	80575.488596	59.974785
2264.428963	80346.834575	59.979790
2263.393958	80120.813072	59.984794
2263.266715	79892.260868	59.989799
2262.074783	79669.057635	59.994804
2261.331277	79443.770442	59.999809
2261.224834	79210.653290	60.004814
2260.058894	78983.815783	60.009818
2259.307703	78768.315363	60.014823
2258.685638	78549.533167	60.019828
2258.105398	78323.776046	60.024833
2257.314236	78096.179145	60.029838
2256.649236	77875.427496	60.034842
2256.262805	77642.999834	60.039847
2255.300189	77432.103055	60.044852
2254.746708	77212.823633	60.049857
2254.052690	76981.554828	60.054862
2253.323282	76765.070830	60.059866
2252.836430	76542.594471	60.064871
2252.095311	76335.722832	60.069876
2251.499353	76106.900548	60.074881
2250.757841	75877.457635	60.079886
2249.822219	75659.567122	60.084890
2249.558546	75431.650162	60.089895
2248.822799	75224.193411	60.094900
2247.969889	75006.936732	60.099905
2247.502103	74780.675126	60.104910
2246.900377	74557.503802	60.109914
2246.275234	74340.997464	60.114919
2245.563076	74121.016329	60.119924
2244.999832	73892.182233	60.124929
2244.560835	73668.684510	60.129934
2243.647847	73446.031032	60.134938
2243.044212	73223.907479	60.139943
2242.302469	73006.185959	60.144948
2241.582423	72773.765723	60.149953
2241.121642	72552.602585	60.154958
2240.304212	72333.056883	60.159962
2239.853682	72103.889591	60.164967
2238.959786	71888.079552	60.169972
2238.489134	71649.316965	60.174977
2237.754580	71425.137372	60.179982
2236.787660	71212.247575	60.184986
2236.585150	70985.068278	60.189991
2235.752292	70751.365625	60.194996
2235.117057	70533.970995	60.200001
2234.664742	70307.548556	60.205006
2233.745035	70081.424545	60.210010
2233.196324	69844.457049	60.215015
2232.387673	69634.257547	60.220020
2231.717220	69407.614010	60.225025
2231.331056	69176.829872	60.230030
2230.352433	68953.572157	60.235034
2229.687710	68727.663968	60.240039
2228.829704	68510.225692	60.245044
2228.248401	68289.484065	60.250049
2227.713896	68077.395652	60.255054
2226.899663	67851.913983	60.260058
2226.522976	67621.210026	60.265063
2225.472671	67408.286005	60.270068
2224.882998	67174.574724	60.275073
2224.445733	66955.491042	60.280078
2223.785990	66734.000485	60.285082
2223.508110	66505.194074	60.290087
2222.447288	66288.832425	60.295092
2221.811951	66069.217030	60.300097
2221.197030	65836.213024	60.305102
2220.295318	65620.587243	60.310106
2219.937059	65395.204310	60.315111
2218.843333	65177.387961	60.320116
2218.228860	64957.512775	60.325121
2217.786181	64734.782187	60.330126
2216.916422	64521.519380	60.335130
2216.447863	64294.165771	60.340135
2215.960266	64080.628783	60.345140
2214.984337	63852.879627	60.350145
2214.393386	63628.719484	60.355150
2213.483967	63406.068879	60.360154
2213.091677	63190.953175	60.365159
2212.334048	62976.337921	60.370164
2211.361772	62753.125538	60.375169
2211.142251	62523.648142	60.380174
2210.358353	62313.157081	60.385178
2209.614282	62110.598848	60.390183
2208.923952	61877.981090	60.395188
2208.079061	61664.103654	60.400193
2207.588526	61448.193837	60.405198
2207.127658	61227.422410	60.410202
2206.205944	61014.102688	60.415207
2205.615303	60799.574242	60.420212
2204.869752	60585.531822	60.425217
2204.480876	60361.542862	60.430222
2203.586277	60151.014318	60.435226
2203.134393	59924.175758	60.440231
2202.078825	59709.553062	60.445236
2201.636632	59491.214291	60.450241
2200.893677	59275.160533	60.455246
2200.325893	59066.130716	60.460250
2199.756477	58848.303927	60.465255
2198.812779	58632.694601	60.470260
2198.385466	58415.632146	60.475265
2198.106394	58199.415971	60.480270
2197.053025	57977.779759	60.485274
2196.698596	57758.013528	60.490279
2195.735327	57553.311018	60.495284
2195.128932	57330.184182	60.500289
2194.663576	57100.650660	60.505294
2193.436532	56892.344869	60.510298
2193.281548	56666.616113	60.515303
2192.372000	56462.600773	60.520308
2191.663293	56249.868266	60.525313
2191.082463	56029.373586	60.530318
2190.468547	55818.938179	60.535322
2189.709710	55593.884836	60.540327
2189.135751	55373.643775	60.545332
2188.465829	55163.547556	60.550337
2188.047242	54943.983235	60.555342
2187.155791	54733.281499	60.560346
2186.720856	54499.044496	60.565351
2185.911131	54289.145042	60.570356
2185.004258	54076.162205	60.575361
2184.739001	53850.982364	60.580366
2183.993856	53640.940886	60.585370
2183.253241	53411.519283	60.590375
2182.483853	53203.160658	60.595380
2181.650261	52983.135158	60.600385
2181.132723	52768.900260	60.605390
2180.572304	52555.772681	60.610394
2179.929808	52330.506970	60.615399
2179.002225	52119.553281	60.620404
2178.502034	51906.607311	60.625409
2177.688827	51685.800145	60.630414
2176.965494	51480.355493	60.635418
2176.608595	51257.570104	60.640423
2175.834988	51053.172925	60.645428
2175.372456	50843.302582	60.650433
2174.679744	50620.916882	60.655438
2173.812202	50409.850293	60.660442
2173.268066	50187.769103	60.665447
2172.737143	49971.968661	60.670452
2171.516895	49763.759246	60.675457
2171.438426	49539.891145	60.680462
2170.701743	49326.567176	60.685466
2169.756999	49112.937091	60.690471
2169.431086	48905.231702	60.695476
2168.493406	48683.421446	60.700481
2167.751582	48466.021288	60.705486
2166.732351	48262.612376	60.710490
2166.433780	48041.044076	60.715495
2165.691674	47842.252593	60.720500
2165.170378	47638.224579	60.725505
2164.837251	47420.816674	60.730510
2163.804899	47216.042642	60.735514
2163.276161	46988.248058	60.740519
2162.451911	46778.093878	60.745524
2161.849221	46568.447956	60.750529
2161.021439	46361.785111	60.755534
2160.295583	46160.966577	60.760538
2159.838313	45940.110866	60.765543
2159.139009	45725.995597	60.770548
2158.379927	45523.579637	60.775553
2157.787458	45313.510557	60.780558
2157.001658	45095.874201	60.785562
2156.424662	44888.040777	60.790567
2155.764718	44678.806032	60.795572
2155.144641	44478.663659	60.800577
2154.462271	44265.234072	60.805582
2153.618969	44059.011992	60.810586
2153.050242	43843.061507	60.815591
2152.183502	43643.571919	60.820596
2151.545576	43435.449196	60.825601
2150.946723	43233.236765	60.830606
2150.335995	43031.493465	60.835610
2149.840334	42821.929220	60.840615
2148.922515	42614.110582	60.845620
2148.024887	42405.756785	60.850625
2147.565044	42202.661493	60.855630
2146.440573	42008.133294	60.860634
2146.139715	41808.922902	60.865639
2145.437633	41601.037943	60.870644
2144.646715	41402.564577	60.875649
2144.019868	41197.758887	60.880654
2143.316021	41010.723375	60.885658
2142.781790	40811.454022	60.890663
2141.803682	40604.934003	60.895668
2141.089563	40410.323975	60.900673
2140.782263	40217.147248	60.905678
2139.954356	40026.572225	60.910682
2138.984281	39818.560046	60.915687
2138.563532	39631.410870	60.920692
2137.732603	39442.311542	60.925697
2137.428690	39242.143317	60.930702
2136.731624	39058.670877	60.935706
2135.686445	38858.714863	60.940711
2135.215402	38673.305751	60.945716
2134.498761	38477.576749	60.950721
2133.850276	38277.485587	60.955726
2133.138910	38094.435244	60.960730
2132.482653	37899.873116	60.965735
2131.700884	37715.850030	60.970740
2130.966404	37530.912504	60.975745
2130.520689	37344.717176	60.980750
2129.774959	37158.686885	60.985754
2128.899355	36966.653594	60.990759
2128.507698	36779.931112	60.995764
2127.506978	36599.729590	61.000769
2127.028762	36393.952739	61.005774
2126.190198	36219.685452	61.010778
2125.979798	36033.737533	61.015783
2125.047742	35839.034249	61.020788
2124.234429	35660.328844	61.025793
2123.481972	35470.162905	61.030798
2122.626884	35300.945027	61.035802
2121.994031	35117.336037	61.040807
2121.275213	34939.437294	61.045812
2120.451008	34766.636884	61.050817
2119.820422	34580.239100	61.055822
2118.831944	34413.524808	61.060826
2118.214051	34242.329706	61.065831
2117.661726	34073.807952	61.070836
2116.747369	33915.603834	61.075841
2116.170893	33743.632872	61.080846
2115.122082	33581.388465	61.085850
2114.522046	33419.469532	61.090855
2113.626788	33253.641802	61.095860
2112.818340	33108.370094	61.100865
2112.035757	32945.819413	61.105870
2111.256160	32801.908051	61.110874
2110.599261	32652.330482	61.115879
2109.837223	32500.602793	61.120884
2108.976526	32361.943601	61.125889
2108.196655	32217.852463	61.130894
2107.251474	32073.923129	61.135898
2106.824885	31931.499319	61.140903
2105.817932	31806.712389	61.145908
2104.869915	31671.487694	61.150913
2104.564160	31536.233314	61.155918
2103.901180	31417.205122	61.160922
2103.026895	31278.547699	61.165927
2102.329767	31153.700751	61.170932
2101.418230	31022.067291	61.175937
2100.879579	30895.533266	61.180942
2100.345192	30772.554805	61.185946
2099.782839	30645.645654	61.190951
2099.065269	30537.408817	61.195956
2098.112281	30416.681549	61.200961
2097.908199	30281.342341	61.205966
2096.956486	30171.211061	61.210970
2096.400903	30042.831299	61.215975
2095.595368	29932.122256	61.220980
2095.061077	29804.654243	61.225985
2094.541928	29677.401280	61.230990
2093.746232	29559.937057	61.235994
2093.184555	29438.936867	61.240999
2092.503083	29324.873729	61.246004
2091.502574	29204.268800	61.251009
2090.886695	29079.687023	61.256014
2090.337881	28972.381731	61.261018
2089.395775	28859.047318	61.266023
2089.088213	28737.863489	61.271028
2088.569823	28621.390549	61.276033
2087.869357	28500.480953	61.281038
2086.881516	28388.896538	61.286042
2086.371450	28269.211302	61.291047
2085.682355	28164.880058	61.296052
2084.674122	28060.442135	61.301057
2084.605500	27933.888038	61.306062
2083.642774	27831.842570	61.311066
2082.685231	27724.457113	61.316071
2082.096653	27609.260099	61.321076
2081.366874	27497.159022	61.326081
2080.939145	27388.527410	61.331086
2080.126405	27285.136139	61.336090
2079.707737	27164.659390	61.341095
2078.993872	27064.130604	61.346100
2078.105480	26960.263687	61.351105
2077.713699	26852.866908	61.356110
2077.038165	26751.837942	61.361114
2076.270252	26644.383750	61.366119
2075.607205	26526.324059	61.371124
2074.679697	26420.447954	61.376129
2074.554987	26317.581629	61.381134
2073.627244	26214.577205	61.386138
2073.052820	26105.531228	61.391143
2072.516801	25992.103460	61.396148
2071.356286	25894.588619	61.401153
2071.250063	25783.112121	61.406158
2070.319021	25680.139282	61.411162
2069.441790	25581.978760	61.416167
2069.025232	25464.621466	61.421172
2068.190762	25364.871932	61.426177
2067.825147	25248.537237	61.431182
2067.004698	25158.210553	61.436186
2066.653148	25051.850851	61.441191
2065.939458	24933.031366	61.446196
2064.849878	24831.977477	61.451201
2064.981166	24721.615817	61.456206
2064.481989	24611.854875	61.461210
2063.499754	24505.199254	61.466215
2062.709741	24391.946288	61.471220
2062.055206	24296.763291	61.476225
2061.231732	24185.429858	61.481230
2060.433421	24076.640888	61.486234
2059.884716	23973.139768	61.491239
2059.770112	23854.994519	61.496244
2058.501307	23752.206127	61.501249
2057.875023	23639.276042	61.506254
2057.373051	23541.303029	61.511258
2056.785966	23437.173391	61.516263
2056.145991	23341.872951	61.521268
2055.230372	23235.721438	61.526273
2054.800415	23121.857298	61.531278
2053.985383	23018.450436	61.536282
2053.573170	22914.615496	61.541287
2053.225320	22803.966428	61.546292
2052.213423	22701.729990	61.551297
2051.178476	22591.893442	61.556302
2050.657928	22480.198514	61.561306
2050.288001	22369.236164	61.566311
2049.412391	22278.844516	61.571316
2048.651178	22182.144959	61.576321
2048.461500	22062.052400	61.581326
2047.689789	21958.123622	61.586330
2046.936238	21845.453885	61.591335
2046.267528	21738.725202	61.596340
2045.184760	21641.374056	61.601345
2044.664401	21530.685437	61.606350
2043.826166	21434.389577	61.611354
2043.318438	21322.711827	61.616359
2042.844177	21226.630307	61.621364
2041.719986	21133.289730	61.626369
2041.345817	21025.671104	61.631374
2040.342789	20930.783078	61.636378
2039.921720	20839.815881	61.641383
2039.238228	20729.274043	61.646388
2038.657838	20637.028933	61.651393
2038.129670	20531.336226	61.656398
2037.493954	20433.484967	61.661402
2036.871433	20335.035325	61.666407
2036.299620	20231.687036	61.671412
2035.066154	20123.249271	61.676417
2034.637966	20028.712076	61.681422
2033.873693	19933.035412	61.686426
2033.332906	19833.360069	61.691431
2033.021445	19737.097578	61.696436
2031.880308	19643.296796	61.701441
2031.281238	19529.373248	61.706446
2030.372777	19440.175113	61.711450
2029.821463	19343.965728	61.716455
2029.314772	19252.073510	61.721460
2028.582444	19152.451442	61.726465
2027.995642	19059.365546	61.731470
2027.306415	18973.250977	61.736474
2026.635890	18881.321408	61.741479
2026.134691	18775.500056	61.746484
2025.352421	18689.035898	61.751489
2024.589287	18593.595784	61.756494
2023.666127	18507.355514	61.761498
2022.954006	18414.690045	61.766503
2022.018441	18322.247290	61.771508
2021.520445	18238.494104	61.776513
2020.951221	18142.590598	61.781518
2020.323850	18054.119943	61.786522
2019.488510	17968.696437	61.791527
2018.958056	17885.984841	61.796532
2017.708306	17799.972805	61.801537
2017.043288	17717.913020	61.806542
2016.456632	17638.448658	61.811546
2015.804057	17557.557257	61.816551
2015.554025	17485.236496	61.821556
2014.320785	17402.399418	61.826561
2014.207366	17316.326161	61.831566
2013.211468	17244.731143	61.836570
2012.617328	17155.372654	61.841575
2012.197273	17077.402317	61.846580
2011.493615	16998.278313	61.851585
2010.918320	16920.399709	61.856590
2010.291523	16836.764498	61.861594
2009.528807	16753.963567	61.866599
2008.762232	16667.012236	61.871604
2007.879407	16597.371921	61.876609
2007.464871	16511.690137	61.881614
2006.315770	16443.433887	61.886618
2005.601824	16369.316845	61.891623
2005.524667	16288.347649	61.896628
2004.699322	16217.317586	61.901633
2004.177127	16140.946848	61.906638
2003.199501	16077.426077	61.911642
2002.925027	15982.776335	61.916647
2002.255356	15901.007509	61.921652
2001.227703	15829.518010	61.926657
2000.444280	15740.656515	61.931662
1999.777122	15673.234503	61.936666
1999.169062	15596.935334	61.941671
1998.659030	15525.932606	61.946676
1997.945906	15462.514663	61.951681
1997.550779	15377.491402	61.956686
1996.600111	15311.341350	61.961690
1996.058630	15231.105310	61.966695
1995.786827	15154.320067	61.971700
1994.498526	15082.664663	61.976705
1994.109845	15005.398504	61.981710
1993.533399	14940.640656	61.986714
1992.511342	14862.653115	61.991719
1991.784078	14788.198901	61.996724
1991.226036	14716.830451	62.001729
1990.782224	14640.580789	62.006734
1989.970032	14578.525631	62.011738
1989.408941	14504.911737	62.016743
1988.780133	14427.613979	62.021748
1988.088622	14376.549905	62.026753
1987.604390	14298.411603	62.031758
1987.071214	14216.279540	62.036762
1986.224485	14143.441376	62.041767
1985.410076	14076.661094	62.046772
1984.820826	14005.104486	62.051777
1984.116454	13927.292263	62.056782
1983.565908	13858.999178	62.061786
1982.675328	13786.363918	62.066791
1982.068094	13710.815744	62.071796
1981.029388	13645.686287	62.076801
1980.398062	13571.641329	62.081806
1979.922308	13511.336878	62.086810
1979.213419	13447.287731	62.091815
1978.579699	13376.883285	62.096820
1977.653308	13303.543460	62.101825
1977.268191	13247.217883	62.106830
1976.614410	13187.844313	62.111834
1975.914091	13118.338868	62.116839
1975.605763	13047.578264	62.121844
1975.022833	12987.770835	62.126849
1974.405311	12915.987550	62.131854
1973.458683	12849.598706	62.136858
1972.921258	12781.500193	62.141863
1972.365615	12705.374291	62.146868
1971.537347	12634.092176	62.151873
1970.876784	12566.283665	62.156878
1970.223936	12494.916948	62.161882
1969.177922	12425.999538	62.166887
1969.045526	12346.260358	62.171892
1968.021273	12296.272762	62.176897
1967.406946	12229.076704	62.181902
1966.869077	12157.938739	62.186906
1966.085703	12100.582137	62.191911
1965.962123	12031.245493	62.196916
1964.855430	11960.549499	62.201921
1964.503519	11887.103319	62.206926
1963.405788	11822.849882	62.211930
1962.699571	11761.766379	62.216935
1962.431309	11690.986898	62.221940
1961.558688	11621.992944	62.226945
1960.866362	11548.003701	62.231950
1960.418932	11489.904835	62.236954
1959.691006	11422.355950	62.241959
1958.799506	11345.738683	62.246964
1957.720834	11293.311336	62.251969
1957.273223	11224.252128	62.256974
1956.998663	11163.658429	62.261978
1956.419079	11095.784646	62.266983
1955.635381	11031.512933	62.271988
1954.893615	10962.473201	62.276993
1953.836058	10898.729417	62.281998
1953.347050	10839.281268	62.287002
1952.795593	10777.571169	62.292007
1952.670478	10702.460583	62.297012
1951.752798	10639.956994	62.302017
1951.211627	10573.923271	62.307022
1950.334508	10509.357919	62.312026
1949.386972	10443.359678	62.317031
1948.950870	10374.410028	62.322036
1948.104894	10317.060651	62.327041
1947.549617	10248.047251	62.332046
1946.656427	10192.242482	62.337050
1946.035181	10128.810839	62.342055
1945.595424	10066.041246	62.347060
1944.786010	10008.330209	62.352065
1944.538458	9938.736396	62.357070
1943.635037	9872.839379	62.362074
1942.594696	9815.648215	62.367079
1942.169295	9747.396031	62.372084
1941.512989	9690.867114	62.377089
1940.961466	9625.585187	62.382094
1940.340841	9569.380075	62.387098
1939.218884	9515.261553	62.392103
1938.989872	9452.595982	62.397108
1937.961530	9400.404719	62.402113
1937.489786	9328.019215	62.407118
1936.843584	9273.091506	62.412122
1936.163541	9212.569206	62.417127
1935.747206	9147.488809	62.422132
1934.738190	9089.803512	62.427137
1934.144995	9025.206165	62.432142
1933.385256	8962.335355	62.437146
1932.806642	8900.655398	62.442151
1932.122001	8843.381497	62.447156
1931.190977	8786.938246	62.452161
1930.879575	8732.259570	62.457166
1930.486509	8673.197241	62.462170
1929.805373	8616.881434	62.467175
1929.326206	8546.414462	62.472180
1928.303963	8497.595739	62.477185
1927.851248	8425.181190	62.482190
1926.972368	8347.897500	62.487194
1926.332371	8295.521820	62.492199
1925.932009	8230.037750	62.497204
1924.994410	8181.749010	62.502209
1924.438506	8110.088034	62.507214
1923.770549	8051.975100	62.512218
1923.027956	7995.714381	62.517223
1922.338707	7944.251056	62.522228
1921.970315	7885.965779	62.527233
1921.182436	7820.220379	62.532238
1920.288694	7757.399173	62.537242
1919.380045	7697.801667	62.542247
1919.189156	7638.675035	62.547252
1918.451039	7583.170526	62.552257
1917.857550	7520.383912	62.557262
1917.439321	7450.141599	62.562266
1916.364994	7397.890078	62.567271
1915.713977	7336.044251	62.572276
1915.188327	7284.846749	62.577281
1914.463511	7222.970507	62.582286
1913.519624	7169.959118	62.587290
1912.950570	7110.800729	62.592295
1912.360441	7048.585129	62.597300
1911.472305	7002.357604	62.602305
1911.130805	6938.367503	62.607310
1910.400387	6881.266160	62.612314
1909.989811	6824.460966	62.617319
1909.236685	6760.533814	62.622324
1908.390490	6706.403393	62.627329
1907.532203	6653.105739	62.632334
1907.275753	6590.241932	62.637338
1906.521725	6538.951511	62.642343
1906.136282	6475.328505	62.647348
1905.143080	6411.522215	62.652353
1904.363363	6356.682823	62.657358
1903.981778	6299.097642	62.662362
1902.710882	6246.791449	62.667367
1902.401436	6179.262447	62.672372
1901.904149	6138.283524	62.677377
1901.487272	6079.196582	62.682382
1900.697202	6013.208667	62.687386
1899.913708	5959.134912	62.692391
1899.623026	5898.175752	62.697396
1898.807800	5858.449420	62.702401
1897.912782	5789.044725	62.707406
1897.403795	5731.455151	62.712410
1896.722658	5674.152640	62.717415
1896.012483	5615.242679	62.722420
1895.103369	5555.978818	62.727425
1894.603145	5490.127063	62.732430
1893.897018	5433.223054	62.737434
1892.929016	5388.854248	62.742439
1892.702807	5319.581426	62.747444
1891.609771	5274.734309	62.752449
1890.998652	5213.856439	62.757454
1890.640060	5168.978237	62.762458
1889.649718	5114.135079	62.767463
1889.264698	5064.946866	62.772468
1888.553905	5004.535273	62.777473
1887.897217	4957.117921	62.782478
1887.305318	4896.508059	62.787482
1886.460750	4848.873213	62.792487
1885.805939	4796.128884	62.797492
1885.168628	4739.364907	62.802497
1884.615301	4680.933831	62.807502
1884.066042	4625.089391	62.812506
1883.429926	4570.901880	62.817511
1882.509734	4509.812541	62.822516
1881.843505	4475.021864	62.827521
1881.196895	4405.514035	62.832526
1880.555250	4344.105898	62.837530
1879.688604	4298.750216	62.842535
1879.572671	4239.231640	62.847540
1879.009154	4195.027790	62.852545
1878.084014	4130.860887	62.857550
1877.486070	4070.107892	62.862554
1876.870960	4018.501299	62.867559
1876.212454	3957.684245	62.872564
1875.259366	3910.904895	62.877569
1874.590220	3856.851446	62.882574
1874.107564	3800.736922	62.887578
1873.141851	3759.364959	62.892583
1872.636099	3696.396852	62.897588
1871.990547	3644.096054	62.902593
1870.820717	3599.043043	62.907598
1870.796395	3541.915847	62.912602
1869.993825	3495.150207	62.917607
1869.708331	3431.437671	62.922612
1868.928009	3387.204420	62.927617
1868.085594	3321.490803	62.932622
1867.500804	3264.616127	62.937626
1866.432083	3218.224073	62.942631
1866.107237	3166.047568	62.947636
1865.520031	3115.971288	62.952641
1864.534272	3053.842402	62.957646
1863.940112	3009.939572	62.962650
1863.326200	2957.240297	62.967655
1862.793635	2904.349275	62.972660
1861.986888	2863.985362	62.977665
1860.677212	2814.196737	62.982670
1860.210337	2757.988267	62.987674
1859.806567	2726.100102	62.992679
1859.873956	2665.572993	62.997684
1858.737728	2620.362304	63.002689
1858.252356	2568.453941	63.007694
1857.575680	2511.573905	63.012698
1856.750544	2461.017936	63.017703
1856.217411	2407.154067	63.022708
1855.388327	2358.218899	63.027713
1854.497038	2304.852315	63.032718
1853.878630	2251.535658	63.037722
1853.110519	2210.803869	63.042727
1852.710182	2155.632838	63.047732
1852.249696	2114.772828	63.052737
1851.371052	2068.511970	63.057742
1850.841918	2011.120738	63.062746
1850.111180	1976.249240	63.067751
1849.467811	1920.185567	63.072756
1848.533618	1880.667896	63.077761
1847.822176	1832.193700	63.082766
1847.197188	1778.277337	63.087770
1846.517588	1743.401433	63.092775
1845.882203	1689.633724	63.097780
1845.189368	1637.971367	63.102785
1844.446603	1604.505545	63.107790
1843.654331	1559.240388	63.112794
1842.978551	1514.233665	63.117799
1842.846583	1467.205600	63.122804
1842.202045	1420.460939	63.127809
1841.240496	1378.748886	63.132814
1840.755741	1316.636169	63.137818
1839.763611	1284.426632	63.142823
1839.247684	1240.823449	63.147828
1838.368092	1202.998285	63.152833
1837.686862	1153.797661	63.157838
1837.518327	1111.596159	63.162842
1836.781428	1074.927551	63.167847
1836.372882	1013.536585	63.172852
1835.245821	989.086295	63.177857
1834.397168	936.275456	63.182862
1833.877956	896.432783	63.187866
1833.127865	850.429011	63.192871
1832.851603	806.584848	63.197876
1831.651076	762.341903	63.202881
1831.040912	736.042095	63.207886
1830.424201	690.314140	63.212890
1829.706084	657.721850	63.217895
1829.308731	603.761868	63.222900
1828.363659	563.453109	63.227905
1827.648907	530.149329	63.232910
1826.958726	497.094050	63.237914
1826.194271	452.927902	63.242919
1825.667005	421.589537	63.247924
1824.839794	376.974672	63.252929
1824.107591	349.532685	63.257934
1823.993671	305.791996	63.262938
1822.700929	270.246618	63.267943
1821.940639	249.781994	63.272948
1821.426352	216.913899	63.277953
1820.718031	178.293858	63.282958
1819.907234	142.574500	63.287962
1819.362261	117.495517	63.292967
1818.335968	92.945595	63.297972
1817.247095	77.675140	63.302977
1816.855476	48.183193	63.307982
1816.293408	43.402768	63.312986
1814.641148	42.518686	63.317991
1812.796364	57.990046	63.322996
1811.810533	70.243620	63.328001
1811.882650	71.850187	63.333006
1811.660636	71.391880	63.338010
1810.309667	83.028494	63.343015
1810.599119	78.168049	63.348020
1810.110470	84.570944	63.353025
1809.046608	80.828989	63.358030
1808.564351	79.427968	63.363034
1807.205868	101.245204	63.368039
1807.090941	85.906837	63.373044
1806.494495	76.451382	63.378049
1805.781771	85.827772	63.383054
1805.324335	91.793622	63.388058
1804.796742	92.292178	63.393063
1804.358447	81.748723	63.398068
1803.757656	87.634830	63.403073
1802.908089	87.705107	63.408078
1801.934448	77.842759	63.413082
1801.033879	90.268897	63.418087
1800.293562	89.046050	63.423092
1799.710573	94.833138	63.428097
1799.145494	91.595469	63.433102
1798.935920	86.055730	63.438106
1798.299839	95.495653	63.443111
1797.914275	88.129327	63.448116
1797.030259	92.369885	63.453121
1796.007254	98.047067	63.458126
1795.751621	88.001318	63.463130
1794.389477	93.692925	63.468135
1793.620253	86.996236	63.473140
1792.979889	86.727363	63.478145
1792.900288	86.561841	63.483150
1792.918567	74.826240	63.488154
1791.914584	92.308831	63.493159
1791.327387	82.670556	63.498164
1790.626217	83.393799	63.503169
1789.329143	93.583665	63.508174
1788.905030	89.719630	63.513178
1788.293241	88.017476	63.518183
1787.548077	81.750641	63.523188
1786.865053	84.976826	63.528193
1785.954823	85.960352	63.533198
1785.533655	84.516518	63.538202
1784.632430	91.847541	63.543207
1784.477528	87.161731	63.548212
1784.192569	84.120865	63.553217
1783.075750	85.365858	63.558222
1782.724931	80.980824	63.563226
1781.454968	85.161242	63.568231
1781.468058	80.660074	63.573236
1780.666198	80.440504	63.578241
1779.334267	91.761872	63.583246
1779.347306	79.222840	63.588250
1778.728097	90.074634	63.593255
1778.183579	83.900522	63.598260
1777.060722	83.750848	63.603265
1776.402582	93.047616	63.608270
1776.160649	77.906053	63.613274
1775.444968	90.738085	63.618279
1774.680112	93.808532	63.623284
1773.146516	86.772749	63.628289
1773.100309	94.083124	63.633294
1772.833656	79.571547	63.638298
1771.896282	87.482332	63.643303
1771.511379	88.585874	63.648308
1770.771099	85.663044	63.653313
1770.310671	88.213632	63.658318
1769.656522	85.267664	63.663322
1768.008319	87.160028	63.668327
1767.538179	91.328564	63.673332
1767.296501	85.811274	63.678337
1766.754282	78.717422	63.683342
1766.267685	80.985155	63.688346
1765.795931	90.105665	63.693351
1765.137905	84.949387	63.698356
1763.743451	75.737366	63.703361
1763.266609	86.962374	63.708366
1763.131363	86.237976	63.713370
1761.608071	88.119969	63.718375
1761.625874	85.217111	63.723380
1761.059817	81.189542	63.728385
1759.599043	85.758245	63.733390
1759.481273	76.662039	63.738394
1759.114582	82.679713	63.743399
1758.233649	75.119250	63.748404
1757.362278	87.408292	63.753409
1756.422937	90.960621	63.758414
1756.310213	81.713798	63.763418
1755.477350	84.985862	63.768423
1754.645785	85.676204	63.773428
1754.149103	89.554061	63.778433
1753.576164	87.260686	63.783438
1752.933527	88.834098	63.788442
1751.942638	90.637859	63.793447
1751.854152	87.116357	63.798452
1750.775711	90.511002	63.803457
1750.102880	91.038940	63.808462
1749.893286	83.766110	63.813466
1748.867413	88.051286	63.818471
1748.145302	85.239121	63.823476
1747.734804	84.025416	63.828481
1746.961892	95.778428	63.833486
1746.673244	88.453494	63.838490
1745.942162	84.895266	63.843495
1745.620564	83.184887	63.848500
1744.692185	82.726795	63.853505
1743.283527	89.718934	63.858510
1742.878960	77.667281	63.863514
1742.467933	91.632094	63.868519
1741.801811	83.301070	63.873524
1740.983108	82.721482	63.878529
1739.937672	86.161352	63.883534
1739.467086	88.024417	63.888538
1739.175265	83.035499	63.893543
1738.376850	82.944707	63.898548
1737.828549	80.863471	63.903553
1736.882735	85.053934	63.908558
1736.585818	89.041997	63.913562
1735.767135	91.597444	63.918567
1735.384331	91.538423	63.923572
1734.789533	84.408772	63.928577
1733.802752	88.914830	63.933582
1733.775849	87.588168	63.938586
1732.809156	93.497704	63.943591
1731.495935	84.626041	63.948596
1730.933354	85.497603	63.953601
1730.023132	83.883861	63.958606
1730.274875	79.124018	63.963610
1729.256501	85.365041	63.968615
1728.230147	76.247550	63.973620
1727.895767	84.601910	63.978625
1726.995854	90.486648	63.983630
1726.641300	80.735754	63.988634
1726.110824	79.798155	63.993639
1725.674014	89.838806	63.998644
1725.259452	83.022740	64.003649
1724.297305	85.873790	64.008654
1723.423759	85.542618	64.013658
1722.342249	80.803699	64.018663
1721.532828	75.064344	64.023668
1721.007965	83.124097	64.028673
1720.322541	82.972788	64.033678
1720.194394	79.665750	64.038682
1719.650254	88.233201	64.043687
1718.981037	94.114421	64.048692
1718.636187	89.659061	64.053697
1717.551848	91.758378	64.058702
1716.253755	93.249812	64.063706
1715.470861	89.179418	64.068711
1715.662336	86.463448	64.073716
1714.875564	82.657027	64.078721
1714.072683	85.793452	64.083726
1713.567699	91.853597	64.088730
1712.800471	89.652591	64.093735
1712.425791	89.857216	64.098740
1711.932326	82.217885	64.103745
1710.571489	92.116704	64.108750
1709.900061	83.315017	64.113754
1708.889013	86.159646	64.118759
1708.926578	92.616181	64.123764
1707.978834	90.658315	64.128769
1707.035653	99.267072	64.133774
1706.928754	77.512302	64.138778
1706.253074	87.657123	64.143783
1705.551279	89.331406	64.148788
1705.290176	90.317522	64.153793
1704.733618	94.075585	64.158798
1704.223988	94.744775	64.163802
1702.793150	86.647181	64.168807
1702.107969	86.883775	64.173812
1701.225918	93.402785	64.178817
1700.673128	96.466379	64.183822
1700.182293	82.406747	64.188826
1699.726804	82.805560	64.193831
1699.167008	87.757910	64.198836
1698.818544	81.987929	64.203841
1697.255902	92.111196	64.208846
1696.811220	88.004439	64.213850
1695.585058	86.235880	64.218855
1695.031035	80.593167	64.223860
1695.348544	75.300898	64.228865
1694.134423	87.128718	64.233870
1693.828942	74.276009	64.238874
1693.265210	83.978842	64.243879
1692.757615	90.361108	64.248884
1692.424056	73.885806	64.253889
1691.477415	91.635279	64.258894
1690.791537	86.145973	64.263898
1689.936200	95.343186	64.268903
1688.657761	88.020925	64.273908
1688.255437	82.789365	64.278913
1687.338483	93.032439	64.283918
1686.955582	95.187520	64.288922
1686.143851	90.132949	64.293927
1685.072608	78.997766	64.298932
1685.314372	81.755387	64.303937
1684.684829	84.536277	64.308942
1683.742842	82.208495	64.313946
1683.180421	88.112182	64.318951
1682.406895	79.479690	64.323956
1682.054455	84.162560	64.328961
1681.441382	92.581692	64.333966
1680.297524	80.475585	64.338970
1679.543265	84.473212	64.343975
1678.964498	73.993111	64.348980
1678.806364	83.114275	64.353985
1677.914952	87.187304	64.358990
1677.791329	80.203613	64.363994
1676.985915	83.747311	64.368999
1675.438084	86.134729	64.374004
1674.937709	79.177763	64.379009
1673.788694	86.193349	64.384014
1673.591976	73.932084	64.389018
1673.151345	86.256807	64.394023
1672.580660	84.781547	64.399028
1671.989963	78.696804	64.404033
1671.513596	82.167738	64.409038
1671.177376	80.407652	64.414042
1670.027502	76.917546	64.419047
1669.299546	77.947854	64.424052
1668.785336	80.133254	64.429057
1668.077602	81.100426	64.434062
1667.879537	74.011866	64.439066
1666.688389	75.708690	64.444071
1665.878431	81.240103	64.449076
1665.237563	73.862326	64.454081
1664.200809	83.693913	64.459086
1664.108072	74.221579	64.464090
1663.559039	83.658725	64.469095
1662.948702	80.565479	64.474100
1662.285435	74.085407	64.479105
1661.277428	79.066374	64.484110
1660.527333	80.648989	64.489114
1659.769758	74.855690	64.494119
1659.324093	83.019567	64.499124
1658.855695	78.222717	64.504129
1658.263639	77.402148	64.509134
1657.590425	78.540461	64.514138
1656.234905	83.655479	64.519143
1655.536023	87.521311	64.524148
1655.654958	78.576759	64.529153
1654.796347	87.433868	64.534158
1654.377118	74.903593	64.539162
1653.969986	79.598305	64.544167
1653.072585	79.256753	64.549172
1652.306149	60.129951	64.554177
1651.362755	76.472234	64.559182
1650.841047	68.283895	64.564186
1650.262426	76.472041	64.569191
1649.310119	80.143158	64.574196
1648.598618	74.489204	64.579201
1647.654852	82.076178	64.584206
1647.629758	76.163380	64.589210
1646.664207	83.711237	64.594215
1646.144670	84.109194	64.599220
1645.771418	78.671174	64.604225
1645.062097	89.076819	64.609230
1644.565311	74.970849	64.614234
1643.544244	81.217056	64.619239
1642.665366	78.480290	64.624244
1642.265069	70.999652	64.629249
1641.697818	75.733991	64.634254
1641.446574	75.679318	64.639258
1640.119173	72.097576	64.644263
1638.928769	78.006400	64.649268
1638.512583	70.290164	64.654273
1638.062114	71.487717	64.659278
1637.536532	73.608695	64.664282
1637.222773	74.734070	64.669287
1636.421571	80.970586	64.674292
1635.968739	76.403085	64.679297
1635.375392	82.669664	64.684302
1634.317767	70.813249	64.689306
1633.469170	76.541622	64.694311
1632.755063	84.934226	64.699316
1632.625973	75.691601	64.704321
1632.186476	83.367215	64.709326
1631.303756	74.709513	64.714330
1630.142919	84.573436	64.719335
1629.329971	73.742615	64.724340
1628.844346	78.981239	64.729345
1628.071410	88.611657	64.734350
1627.941895	84.385465	64.739354
1627.597839	84.675125	64.744359
1626.439234	81.847179	64.749364
1625.491536	77.527027	64.754369
1624.478412	80.673218	64.759374
1624.299239	73.739362	64.764378
1623.809814	83.515555	64.769383
1623.157581	83.666510	64.774388
1622.803619	69.049002	64.779393
1621.867235	89.403597	64.784398
1621.169852	80.650221	64.789402
1620.724199	81.492193	64.794407
1620.007613	79.393563	64.799412
1619.532480	81.255791	64.804417
1618.342615	87.852104	64.809422
1617.589838	90.094335	64.814426
1617.093914	72.960441	64.819431
1616.555889	90.309119	64.824436
1616.290454	73.783594	64.829441
1615.280346	84.307986	64.834446
1614.681721	83.111573	64.839450
1613.816629	75.968130	64.844455
1613.007558	86.219310	64.849460
1612.598466	74.729820	64.854465
1611.826149	84.800117	64.859470
1611.488585	78.429172	64.864474
1610.137422	83.210776	64.869479
1609.118687	80.682323	64.874484
1609.106593	76.908997	64.879489
1608.690001	80.542335	64.884494
1608.223670	84.088956	64.889498
1607.573458	83.780693	64.894503
1607.037764	85.179452	64.899508
1605.952215	76.667523	64.904513
1605.203576	82.715922	64.909518
1604.453581	82.095499	64.914522
1603.741671	83.635794	64.919527
1603.501099	83.724511	64.924532
1603.345547	79.076675	64.929537
1602.031398	88.375176	64.934542
1601.271082	80.970659	64.939546
1601.003891	79.622248	64.944551
1599.973030	83.717453	64.949556
1599.456034	76.157589	64.954561
1598.594146	86.123845	64.959566
1597.391534	81.743273	64.964570
1596.985902	73.186417	64.969575
1596.754857	84.421271	64.974580
1596.697301	76.581836	64.979585
1595.840573	86.859515	64.984590
1594.810920	79.204472	64.989594
1593.871557	85.018241	64.994599
1593.151738	82.410767	64.999604
1593.032328	82.874481	65.004609
1592.074459	83.701635	65.009614
1591.639295	70.658243	65.014618
1590.741650	78.758306	65.019623
1589.707112	87.913042	65.024628
1589.377649	71.842406	65.029633
1588.747788	83.224197	65.034638
1588.435576	75.308523	65.039642
1587.770723	77.368056	65.044647
1586.502911	84.631208	65.049652
1585.845795	81.838731	65.054657
1585.272302	88.885924	65.059662
1585.077651	79.295746	65.064666
1584.711557	81.334625	65.069671
1583.565912	89.945611	65.074676
1582.694689	75.545905	65.079681
1582.266935	87.479073	65.084686
1581.598633	89.196952	65.089690
1581.509000	83.212407	65.094695
1579.613610	83.851034	65.099700
1579.227190	83.668029	65.104705
1578.560357	81.310767	65.109710
1578.185074	76.726228	65.114714
1577.714069	80.647339	65.119719
1577.055630	81.168303	65.124724
1576.903160	75.636875	65.129729
1575.550621	83.621553	65.134734
1574.644758	81.259688	65.139738
1574.298017	77.706690	65.144743
1573.413233	77.705365	65.149748
1573.620584	81.197002	65.154753
1572.358565	86.729297	65.159758
1571.493709	82.112149	65.164762
1570.794745	77.998511	65.169767
1570.175540	80.837707	65.174772
1569.906035	69.991541	65.179777
1569.172243	77.516790	65.184782
1568.272182	77.647206	65.189786
1567.787660	75.917005	65.194791
1566.899977	76.006031	65.199796
1566.701670	73.862924	65.204801
1565.869293	81.176753	65.209806
1564.759964	81.744124	65.214810
1564.320022	71.704062	65.219815
1563.576835	79.793786	65.224820
1563.183427	70.940103	65.229825
1562.892563	82.504585	65.234830
1561.794276	73.855930	65.239834
1561.088671	74.889024	65.244839
1560.120406	79.324385	65.249844
1560.032472	68.916159	65.254849
1559.425616	76.801293	65.259854
1558.537193	79.960812	65.264858
1557.813859	78.585527	65.269863
1557.275180	68.581658	65.274868
1556.587944	74.855278	65.279873
1555.197031	78.938314	65.284878
1554.519172	74.135344	65.289882
1554.238594	72.632946	65.294887
1553.959754	75.977894	65.299892
1553.533504	70.177727	65.304897
1552.667206	74.775087	65.309902
1552.038697	78.115666	65.314906
1551.266910	76.030557	65.319911
1550.224542	71.301273	65.324916
1550.033894	78.158327	65.329921
1549.340177	79.344080	65.334926
1549.102068	71.476568	65.339930
1547.808194	75.113675	65.344935
1546.993939	79.444145	65.349940
1546.622078	72.917813	65.354945
1545.986659	79.288861	65.359950
1545.242925	72.145091	65.364954
1544.133027	68.207142	65.369959
1543.280757	83.421631	65.374964
1542.956552	75.757034	65.379969
1542.510650	83.577178	65.384974
1542.152918	84.953981	65.389978
1541.832127	75.235619	65.394983
1540.889007	81.657135	65.399988
1539.983596	81.436746	65.404993
1539.361410	87.747348	65.409998
1538.475720	80.097843	65.415002
1538.305854	79.796858	65.420007
1537.502325	81.668699	65.425012
1536.615160	76.271354	65.430017
1536.083587	79.307948	65.435022
1535.472704	79.736210	65.440026
1534.616166	77.188326	65.445031
1533.506555	80.419266	65.450036
1533.230904	73.384057	65.455041
1532.344008	76.346218	65.460046
1531.985313	78.596820	65.465050
1531.561349	68.809701	65.470055
1531.025774	76.066916	65.475060
1530.649763	70.906909	65.480065
1529.578738	68.069827	65.485070
1528.849758	74.848409	65.490074
1528.118531	73.195263	65.495079
1526.517513	78.210572	65.500084
1526.273522	78.690930	65.505089
1526.306755	74.181844	65.510094
1525.372387	83.076249	65.515098
1525.024776	78.531479	65.520103
1524.127654	81.484230	65.525108
1524.017459	73.681554	65.530113
1522.844158	84.422715	65.535118
1521.959747	81.846146	65.540122
1521.638499	71.643733	65.545127
1520.814415	73.020519	65.550132
1520.647888	77.662822	65.555137
1519.780533	76.061270	65.560142
1518.867197	79.950168	65.565146
1518.506718	76.855108	65.570151
1516.713035	75.460669	65.575156
1516.388510	70.242020	65.580161
1515.577915	76.773373	65.585166
1515.036783	74.470275	65.590170
1514.778683	77.663695	65.595175
1514.608645	87.636737	65.600180
1514.094511	69.357741	65.605185
1513.146880	76.659932	65.610190
1511.821162	71.087851	65.615194
1511.247850	75.190808	65.620199
1510.841425	83.788438	65.625204
1510.343228	66.309596	65.630209
1510.012252	75.248475	65.635214
1509.302801	81.251243	65.640218
1508.585117	71.070823	65.645223
1507.917354	76.854074	65.650228
1507.105071	72.309026	65.655233
1505.842137	79.491007	65.660238
1505.135923	82.489125	65.665242
1504.798716	73.471981	65.670247
1504.055289	78.652237	65.675252
1503.845102	65.358660	65.680257
1503.514106	74.974063	65.685262
1502.501254	69.044765	65.690266
1501.704366	64.273344	65.695271
1501.066340	69.288613	65.700276
1500.663452	62.601644	65.705281
1499.316949	71.252449	65.710286
1498.814176	65.753042	65.715290
1498.238881	76.678307	65.720295
1497.796601	77.973932	65.725300
1497.655970	68.343653	65.730305
1496.476020	72.662857	65.735310
1495.427408	76.131704	65.740314
1495.017554	77.530988	65.745319
1494.466447	70.522210	65.750324
1494.461835	67.891010	65.755329
1492.984323	69.523025	65.760334
1492.150037	76.638474	65.765338
1491.490577	71.826294	65.770343
1490.802135	74.173453	65.775348
1490.812233	72.929229	65.780353
1489.783626	73.564230	65.785358
1489.004043	73.210322	65.790362
1487.979620	70.640247	65.795367
1487.726697	78.524345	65.800372
1487.474735	69.376966	65.805377
1486.783650	76.379774	65.810382
1485.560632	81.295617	65.815386
1484.672087	67.889060	65.820391
1483.919391	73.565961	65.825396
1483.811586	67.175883	65.830401
1483.352635	70.746578	65.835406
1482.962135	70.286689	65.840410
1482.692468	64.303961	65.845415
1481.224441	73.554412	65.850420
1480.675942	64.544047	65.855425
1480.239995	67.540222	65.860430
1478.970121	72.513973	65.865434
1478.231441	66.343997	65.870439
1477.579965	75.699665	65.875444
1477.182867	69.686722	65.880449
1476.548232	67.237641	65.885454
1476.139914	64.522359	65.890458
1475.501308	68.720853	65.895463
1474.673545	72.335964	65.900468
1473.904387	73.754499	65.905473
1473.562689	65.425643	65.910478
1472.385028	72.184070	65.915482
1471.895911	64.205074	65.920487
1471.107222	77.796222	65.925492
1470.951867	71.205539	65.930497
1470.264039	70.280384	65.935502
1469.123873	75.088448	65.940506
1468.438336	70.704625	65.945511
1467.602653	77.661028	65.950516
1467.689581	65.905104	65.955521
1467.013161	68.898493	65.960526
1465.797375	73.702804	65.965530
1465.320323	66.165022	65.970535
1464.294007	70.459824	65.975540
1464.035727	65.342624	65.980545
1463.644302	64.496527	65.985550
1462.912618	71.518405	65.990554
1462.071283	66.530131	65.995559
1461.129304	76.379827	66.000564
1460.603925	70.455083	66.005569
1460.289977	71.206764	66.010574
1459.674203	77.669324	66.015578
1458.862006	68.428052	66.020583
1457.823841	67.698925	66.025588
1457.193932	65.693805	66.030593
1457.061214	64.693054	66.035598
1456.363485	70.149910	66.040602
1455.366066	66.263517	66.045607
1454.803953	78.033527	66.050612
1454.416829	69.462729	66.055617
1453.546170	72.231520	66.060622
1452.546680	72.134923	66.065626
1451.950060	68.935476	66.070631
1451.201993	71.596475	66.075636
1450.486330	73.126366	66.080641
1450.780842	63.248748	66.085646
1450.009647	71.063817	66.090650
1449.005607	62.950614	66.095655
1448.189569	75.193066	66.100660
1447.801145	62.391460	66.105665
1446.813662	68.454191	66.110670
1445.694023	71.718297	66.115674
1445.626637	63.303276	66.120679
1444.960376	66.009623	66.125684
1444.750320	53.900356	66.130689
1443.734713	70.221030	66.135694
1442.689666	63.270268	66.140698
1442.237150	63.518840	66.145703
1441.475497	70.025083	66.150708
1440.960823	61.070859	66.155713
1439.886961	69.161113	66.160718
1438.689336	69.219014	66.165722
1438.590968	73.497243	66.170727
1437.992073	76.948258	66.175732
1437.900980	68.958054	66.180737
1437.420769	71.954961	66.185742
1437.018503	73.944412	66.190746
1436.041368	67.555300	66.195751
1435.129344	64.038549	66.200756
1434.563085	64.771983	66.205761
1433.415219	68.600405	66.210766
1432.447413	63.061379	66.215770
1432.235912	60.021510	66.220775
1431.720432	69.153714	66.225780
1431.324640	72.567721	66.230785
1430.727817	69.188536	66.235790
1429.870542	68.090046	66.240794
1429.358028	69.628658	66.245799
1428.632873	63.286238	66.250804
1427.582598	63.180376	66.255809
1426.768707	66.126235	66.260814
1425.842910	72.981849	66.265818
1425.768020	69.724723	66.270823
1425.214995	69.766918	66.275828
1424.944410	59.116509	66.280833
1423.775796	64.607206	66.285838
1423.119539	65.388062	66.290842
1423.076961	61.126002	66.295847
1421.708219	69.706256	66.300852
1420.789055	63.446713	66.305857
1420.171550	62.825790	66.310862
1419.489116	72.157999	66.315866
1419.479210	64.476599	66.320871
1418.709537	72.731408	66.325876
1417.440342	66.920162	66.330881
1417.261851	72.434855	66.335886
1416.875973	67.115589	66.340890
1416.985937	58.399571	66.345895
1415.946333	60.936599	66.350900
1414.926332	66.786885	66.355905
1414.078740	68.597953	66.360910
1413.066160	68.828308	66.365914
1412.536074	60.966230	66.370919
1411.510893	70.343451	66.375924
1410.626434	65.152314	66.380929
1410.077259	71.282592	66.385934
1409.364406	68.868038	66.390938
1409.274673	57.602256	66.395943
1408.778803	65.791470	66.400948
1408.785549	69.619323	66.405953
1407.686163	63.820519	66.410958
1406.634238	72.052381	66.415962
1406.207281	65.504876	66.420967
1404.762030	65.097518	66.425972
1404.153481	60.351395	66.430977
1403.514046	57.575088	66.435982
1402.897763	64.554979	66.440986
1402.485879	60.717474	66.445991
1402.193307	62.899231	66.450996
1401.774286	60.537329	66.456001
1401.595073	63.439092	66.461006
1400.663054	66.271268	66.466010
1399.414637	64.090074	66.471015
1398.270535	73.852060	66.476020
1397.737190	61.672753	66.481025
1397.210269	69.649282	66.486030
1396.561004	71.853040	66.491034
1396.614095	59.004933	66.496039
1395.380086	73.650897	66.501044
1394.441436	64.800342	66.506049
1394.130223	71.591399	66.511054
1393.365969	68.107947	66.516058
1393.080219	69.943265	66.521063
1391.152585	70.308029	66.526068
1390.874660	65.898871	66.531073
1390.605028	61.997757	66.536078
1390.084564	68.948229	66.541082
1390.133787	61.336284	66.546087
1389.037108	72.822249	66.551092
1388.115237	61.649305	66.556097
1387.371205	68.665275	66.561102
1386.709443	66.212645	66.566106
1386.598180	67.047238	66.571111
1385.155945	61.126319	66.576116
1384.356012	64.459483	66.581121
1383.855842	57.504150	66.586126
1383.306481	69.674260	66.591130
1383.301977	69.378542	66.596135
1382.213266	70.739083	66.601140
1381.524684	67.871243	66.606145
1381.086205	64.578870	66.611150
1380.461702	69.219848	66.616154
1379.851052	60.343976	66.621159
1378.553463	63.841398	66.626164
1377.805662	66.683725	66.631169
1377.737667	58.622053	66.636174
1377.148608	66.231564	66.641178
1376.204417	69.071991	66.646183
1375.194697	69.114247	66.651188
1374.924268	65.845627	66.656193
1374.532401	66.040416	66.661198
1373.604500	70.371646	66.666202
1372.310709	59.486489	66.671207
1371.710278	63.817707	66.676212
1371.285545	62.153741	66.681217
1370.870002	56.528540	66.686222
1370.505476	63.872123	66.691226
1370.117342	55.938611	66.696231
1369.274599	65.748896	66.701236
1368.442786	65.229860	66.706241
1367.788570	62.060092	66.711246
1367.057783	59.750906	66.716250
1366.157920	57.779259	66.721255
1365.153322	68.220829	66.726260
1364.858214	63.156810	66.731265
1364.675615	71.258388	66.736270
1364.067674	70.833080	66.741274
1363.294351	65.151206	66.746279
1362.484723	70.286819	66.751284
1361.954633	72.679802	66.756289
1361.126198	67.107614	66.761294
1360.101222	69.885192	66.766298
1359.821038	68.368563	66.771303
1358.763779	73.390575	66.776308
1358.529252	65.568263	66.781313
1357.584929	66.929518	66.786318
1356.895373	56.381994	66.791322
1356.423277	59.324004	66.796327
1355.398306	73.350120	66.801332
1355.484922	67.575711	66.806337
1354.801572	56.355411	66.811342
1353.871549	67.209335	66.816346
1353.412693	63.798780	66.821351
1352.354367	69.264091	66.826356
1351.651271	71.802849	66.831361
1351.062725	61.370155	66.836366
1350.217009	66.517815	66.841370
1349.999396	57.987915	66.846375
1349.469744	67.256422	66.851380
1348.545304	65.345458	66.856385
1347.925912	63.702976	66.861390
1347.106043	70.172762	66.866394
1346.539806	60.823058	66.871399
1345.465187	66.156917	66.876404
1344.825401	66.181382	66.881409
1344.408516	60.218927	66.886414
1343.859590	65.111250	66.891418
1343.395352	52.479433	66.896423
1342.740624	65.822211	66.901428
1341.746145	60.558705	66.906433
1340.944326	52.181600	66.911438
1340.226959	65.225249	66.916442
1340.119618	58.303678	66.921447
1339.892763	71.269360	66.926452
1338.671882	59.920042	66.931457
1337.978477	69.037961	66.936462
1337.465037	63.767376	66.941466
1336.656541	61.186697	66.946471
1335.473724	65.023867	66.951476
1334.714118	59.333517	66.956481
1334.621609	63.554039	66.961486
1333.782878	64.488505	66.966490
1333.957144	61.563944	66.971495
1332.340223	67.217407	66.976500
1331.984249	58.638540	66.981505
1331.628177	62.656529	66.986510
1330.897002	68.686437	66.991514
1329.799081	62.207765	66.996519
1328.968593	59.409809	67.001524
1328.413902	52.590895	67.006529
1328.091643	60.777747	67.011534
1327.754595	58.390213	67.016538
1326.969843	61.613745	67.021543
1326.314813	56.857688	67.026548
1325.389587	63.836239	67.031553
1324.975244	62.821918	67.036558
1323.786211	60.666017	67.041562
1323.259308	59.070341	67.046567
1322.592164	59.627446	67.051572
1321.936483	59.000000	67.056577
1321.731792	63.940108	67.061582
1320.355922	64.258213	67.066586
1319.831607	60.004932	67.071591
1319.678749	69.801755	67.076596
1318.707322	72.796343	67.081601
1318.640583	62.876804	67.086606
1317.135557	66.025605	67.091610
1316.600613	63.584375	67.096615
1316.002542	62.829500	67.101620
1315.827688	66.132701	67.106625
1314.969131	71.142063	67.111630
1313.810404	73.598719	67.116634
1313.278182	70.161987	67.121639
1312.807342	70.798276	67.126644
1312.205406	71.567370	67.131649
1311.785384	67.393704	67.136654
1310.660422	72.866470	67.141658
1310.027329	62.988080	67.146663
1309.477767	67.801663	67.151668
1308.926711	67.414634	67.156673
1308.609029	63.754562	67.161678
1307.259096	72.257761	67.166682
1307.097097	65.434767	67.171687
1306.619109	65.110241	67.176692
1305.498273	65.636972	67.181697
1304.618297	67.104712	67.186702
1303.860864	69.573270	67.191706
1303.624551	61.487901	67.196711
1303.123770	69.583290	67.201716
1302.304883	69.355537	67.206721
1301.602019	70.673695	67.211726
1300.829206	65.360773	67.216730
1300.583915	64.040456	67.221735
1299.715751	62.590502	67.226740
1298.679323	67.837882	67.231745
1298.059610	55.189792	67.236750
1297.518027	66.650611	67.241754
1297.428801	60.954624	67.246759
1296.230220	69.260297	67.251764
1295.496244	70.477745	67.256769
1295.046321	64.397549	67.261774
1294.156677	65.679169	67.266778
1294.071741	62.198143	67.271783
1292.611930	65.672510	67.276788
1291.906256	65.098752	67.281793
1291.474598	58.738108	67.286798
1290.916244	64.538696	67.291802
1290.588807	66.386958	67.296807
1290.157226	66.137060	67.301812
1288.721038	77.432603	67.306817
1287.739567	62.369333	67.311822
1287.180622	75.308963	67.316826
1286.894314	52.182523	67.321831
1286.388340	68.234547	67.326836
1286.030455	63.973737	67.331841
1285.401613	65.243860	67.336846
1284.175920	71.234126	67.341850
1283.709014	71.655326	67.346855
1283.264871	68.073711	67.351860
1282.688362	60.368864	67.356865
1281.896644	56.484538	67.361870
1280.869896	68.413581	67.366874
1280.369999	65.335999	67.371879
1280.071324	65.325173	67.376884
1279.376845	67.170288	67.381889
1278.490721	58.290939	67.386894
1277.635626	65.860757	67.391898
1277.281527	67.717990	67.396903
1276.419468	65.320891	67.401908
1275.281564	58.479594	67.406913
1275.265138	59.455232	67.411918
1274.561274	64.979332	67.416922
1273.711688	64.239224	67.421927
1273.609495	62.661191	67.426932
1273.037257	65.343168	67.431937
1271.997962	65.276625	67.436942
1271.408208	74.600432	67.441946
1270.736656	62.920962	67.446951
1269.578996	66.798316	67.451956
1268.890754	69.222767	67.456961
1268.866372	58.616830	67.461966
1267.860636	67.467446	67.466970
1266.899793	61.805959	67.471975
1266.356649	67.722407	67.476980
1265.703330	60.800915	67.481985
1265.688127	65.524815	67.486990
1265.531818	67.571379	67.491994
1264.557563	68.569991	67.496999
1263.727940	76.862752	67.502004
1262.212697	77.092660	67.507009
1261.594116	62.354912	67.512014
1261.073052	69.057911	67.517018
1260.798121	60.502445	67.522023
1260.403374	65.540582	67.527028
1259.337472	66.741427	67.532033
1258.624788	63.355480	67.537038
1258.094279	58.884000	67.542042
1257.718970	57.496051	67.547047
1256.313008	67.654532	67.552052
1255.445014	70.090219	67.557057
1255.183012	57.513004	67.562062
1254.652835	66.863606	67.567066
1254.456342	65.748428	67.572071
1253.905237	63.894838	67.577076
1252.761616	69.722255	67.582081
1252.731786	61.156206	67.587086
1251.177864	67.302751	67.592090
1250.247850	61.128586	67.597095
1249.895981	64.064114	67.602100
1249.178777	74.441103	67.607105
1249.225640	72.205430	67.612110
1248.520739	72.655015	67.617114
1247.615547	67.460931	67.622119
1246.862314	67.760504	67.627124
1246.215372	69.973388	67.632129
1245.578525	73.067771	67.637134
1244.599512	67.800270	67.642138
1244.207911	66.895888	67.647143
1243.498419	61.899353	67.652148
1242.871796	70.667622	67.657153
1242.218650	62.405686	67.662158
1241.022037	65.950196	67.667162
1240.626920	67.277786	67.672167
1240.073411	67.905154	67.677172
1239.989853	63.629120	67.682177
1238.827952	63.118456	67.687182
1237.853376	63.016405	67.692186
1237.700934	63.603658	67.697191
1237.375491	64.484926	67.702196
1235.963504	74.746882	67.707201
1235.618528	62.316903	67.712206
1234.803346	75.727792	67.717210
1234.483754	66.509217	67.722215
1233.850587	62.240147	67.727220
1232.457360	64.033949	67.732225
1231.802028	65.999008	67.737230
1231.296516	74.803219	67.742234
1231.258877	66.260488	67.747239
1230.818030	57.315091	67.752244
1229.625478	64.180056	67.757249
1229.028561	59.126203	67.762254
1228.368498	68.282993	67.767258
1227.772187	59.830675	67.772263
1226.833180	55.703281	67.777268
1226.223435	73.211583	67.782273
1225.831789	60.637640	67.787278
1225.060471	63.639865	67.792282
1224.275398	62.615123	67.797287
1223.282751	65.792892	67.802292
1222.948170	69.375386	67.807297
1222.482630	55.597355	67.812302
1221.948931	67.359705	67.817306
1221.167563	65.101184	67.822311
1220.646166	60.096827	67.827316
1219.865084	63.633621	67.832321
1219.182212	63.885744	67.837326
1217.911792	69.488906	67.842330
1217.270179	68.181155	67.847335
1216.856966	66.557962	67.852340
1216.587590	68.373345	67.857345
1216.233188	62.214901	67.862350
1215.025097	66.693236	67.867354
1214.406289	67.540730	67.872359
1214.008987	62.343174	67.877364
1213.175300	66.668935	67.882369
1212.332292	57.765413	67.887374
1211.323133	69.921917	67.892378
1210.931122	59.207284	67.897383
1210.880375	64.939785	67.902388
1209.983841	68.758295	67.907393
1209.024784	60.368395	67.912398
1208.217452	77.037635	67.917402
1207.938805	69.298059	67.922407
1207.495660	64.568268	67.927412
1206.527968	67.421950	67.932417
1206.075053	56.981936	67.937422
1205.452580	64.685094	67.942426
1204.556473	62.935262	67.947431
1203.373326	63.968691	67.952436
1202.552441	65.158983	67.957441
1202.190354	62.616176	67.962446
1201.875615	67.297817	67.967450
1201.303980	63.909960	67.972455
1200.951459	58.691094	67.977460
1199.914706	59.307003	67.982465
1199.581281	53.760248	67.987470
1198.818634	66.847388	67.992474
1197.879679	60.447585	67.997479
1196.768645	66.705084	68.002484
1196.517364	65.409386	68.007489
1196.230939	63.272445	68.012494
1195.505160	64.048643	68.017498
1194.401878	62.940468	68.022503
1193.887478	54.325327	68.027508
1193.203923	68.238839	68.032513
1193.087389	51.175692	68.037518
1191.874952	58.187334	68.042522
1191.049309	63.579429	68.047527
1190.498830	63.018868	68.052532
1190.080590	72.239715	68.057537
1189.928472	56.251407	68.062542
1188.605140	69.060277	68.067546
1187.897240	62.699429	68.072551
1187.230482	59.288856	68.077556
1186.652083	66.239103	68.082561
1186.108414	58.494372	68.087566
1185.016546	63.829454	68.092570
1184.289710	66.916082	68.097575
1184.176093	63.474318	68.102580
1183.591030	72.458340	68.107585
1183.128979	59.812027	68.112590
1182.092177	64.431873	68.117594
1181.516099	59.814693	68.122599
1181.052071	66.336742	68.127604
1179.866846	66.466909	68.132609
1179.301380	56.975213	68.137614
1178.786133	59.053627	68.142618
1178.328252	60.626173	68.147623
1177.736688	55.252937	68.152628
1176.159906	66.823194	68.157633
1175.691657	55.523027	68.162638
1175.147382	63.059211	68.167642
1174.814525	54.877257	68.172647
1174.495911	62.415402	68.177652
1173.717092	67.262310	68.182657
1173.029561	59.371724	68.187662
1172.049450	60.264068	68.192666
1171.823330	60.699037	68.197671
1170.701131	57.453937	68.202676
1169.672878	66.043232	68.207681
1169.643764	55.181016	68.212686
1168.949766	57.119122	68.217690
1168.351084	56.995167	68.222695
1167.261372	59.270596	68.227700
1166.525321	63.404222	68.232705
1166.340138	54.041291	68.237710
1165.719162	59.120143	68.242714
1164.768474	52.805802	68.247719
1164.138191	57.698474	68.252724
1163.476615	57.174511	68.257729
1163.244756	55.136132	68.262734
1162.461125	65.503192	68.267738
1161.297110	63.568898	68.272743
1160.747428	57.627605	68.277748
1160.387810	63.316182	68.282753
1160.093297	55.520798	68.287758
1159.169672	58.607186	68.292762
1158.367212	59.621095	68.297767
1157.794232	61.025868	68.302772
1156.987879	62.355789	68.307777
1156.439868	57.015057	68.312782
1155.520397	63.167987	68.317786
1155.070878	56.537402	68.322791
1154.578444	56.505364	68.327796
1153.472057	68.048134	68.332801
1153.149616	54.108597	68.337806
1152.444566	57.376271	68.342810
1152.010276	57.521069	68.347815
1150.819381	61.640301	68.352820
1149.996039	53.963715	68.357825
1149.376060	55.776512	68.362830
1148.598111	59.514678	68.367834
1148.059517	58.602151	68.372839
1147.810769	60.437913	68.377844
1146.796558	63.541866	68.382849
1145.908825	55.265236	68.387854
1145.324343	61.743365	68.392858
1144.886338	72.522248	68.397863
1144.353763	71.212944	68.402868
1144.046638	64.553404	68.407873
1143.658045	58.894005	68.412878
1142.515458	68.856108	68.417882
1141.994482	61.795337	68.422887
1141.519335	57.392354	68.427892
1140.068104	63.308158	68.432897
1139.411053	54.856070	68.437902
1138.616905	63.334023	68.442906
1138.371128	63.802083	68.447911
1138.426980	64.050283	68.452916
1137.283888	65.520499	68.457921
1136.527784	62.363849	68.462926
1135.655439	60.080403	68.467930
1135.496376	65.894783	68.472935
1134.704559	53.472827	68.477940
1133.595419	65.072809	68.482945
1133.170229	67.676232	68.487950
1132.723085	56.312796	68.492954
1131.959348	62.273806	68.497959
1131.200781	59.784607	68.502964
1130.145690	57.270028	68.507969
1129.927303	60.384613	68.512974
1129.393324	61.909346	68.517978
1128.441955	66.323234	68.522983
1127.815178	61.177963	68.527988
1127.073222	67.733183	68.532993
1126.951852	60.575746	68.537998
1126.113510	62.790712	68.543002
1124.835555	60.571780	68.548007
1124.560273	57.310277	68.553012
1123.975718	60.303325	68.558017
1123.591123	57.992773	68.563022
1122.504963	65.976275	68.568026
1121.687644	60.613727	68.573031
1121.160652	56.572236	68.578036
1120.563474	64.419619	68.583041
1120.349414	57.893520	68.588046
1119.360935	62.699668	68.593050
1118.421861	58.529751	68.598055
1118.401721	61.433032	68.603060
1117.291228	71.546160	68.608065
1116.694627	64.875895	68.613070
1115.919242	63.759759	68.618074
1115.429397	63.120185	68.623079
1115.126330	58.486411	68.628084
1113.867673	63.220414	68.633089
1113.141281	58.113070	68.638094
1112.686873	64.067465	68.643098
1112.156990	57.000237	68.648103
1111.758818	62.261284	68.653108
1110.882237	62.279314	68.658113
1110.165686	63.410462	68.663118
1109.652932	67.065460	68.668122
1108.301329	64.817248	68.673127
1107.635296	57.153505	68.678132
1106.892255	61.786578	68.683137
1106.867995	51.049759	68.688142
1106.418453	59.605372	68.693146
1106.074667	63.883204	68.698151
1105.128424	53.934852	68.703156
1104.100397	63.525503	68.708161
1103.888886	53.174859	68.713166
1102.640004	66.861327	68.718170
1101.636083	65.429881	68.723175
1101.296401	59.158734	68.728180
1100.443509	60.663233	68.733185
1100.497594	59.216474	68.738190
1099.691432	65.725141	68.743194
1098.835854	65.101163	68.748199
1098.153722	55.803093	68.753204
1097.380948	70.768452	68.758209
1096.964920	65.867214	68.763214
1095.898211	69.542515	68.768218
1095.065634	69.517282	68.773223
1094.813997	49.157711	68.778228
1094.232117	61.333010	68.783233
1094.253115	59.068337	68.788238
1093.080481	54.277986	68.793242
1091.916965	59.916236	68.798247
1091.512666	63.363172	68.803252
1091.331876	64.896391	68.808257
1090.273159	58.391104	68.813262
1089.638587	63.451633	68.818266
1089.038116	66.551301	68.823271
1088.379419	61.579855	68.828276
1087.257129	67.561639	68.833281
1086.902083	62.877788	68.838286
1086.563082	64.327361	68.843290
1086.106066	68.151694	68.848295
1085.084415	56.488566	68.853300
1083.916953	65.719776	68.858305
1083.541990	57.058833	68.863310
1082.907597	70.592376	68.868314
1082.534018	70.399520	68.873319
1081.578500	71.018325	68.878324
1080.701888	76.961037	68.883329
1080.299070	65.787680	68.888334
1079.954458	62.716984	68.893338
1078.852922	66.552373	68.898343
1078.314352	59.797197	68.903348
1077.371270	66.466421	68.908353
1076.900359	62.811837	68.913358
1076.409284	71.076019	68.918362
1075.944372	66.414376	68.923367
1075.209158	60.062644	68.928372
1074.365940	60.193653	68.933377
1073.898612	59.823321	68.938382
1073.118556	59.931667	68.943386
1072.006817	67.504514	68.948391
1071.445263	60.827113	68.953396
1070.842873	61.361366	68.958401
1070.745017	65.242112	68.963406
1070.115013	63.514657	68.968410
1068.895281	66.410055	68.973415
1068.916796	54.040105	68.978420
1068.128469	56.783301	68.983425
1067.543870	57.713696	68.988430
1066.213555	51.160164	68.993434
1065.499694	57.256757	68.998439
1065.410932	52.333436	69.003444
1064.433473	64.631589	69.008449
1063.778983	61.537648	69.013454
1062.966768	64.491228	69.018458
1062.778991	63.000939	69.023463
1062.451595	57.514752	69.028468
1061.079064	65.305705	69.033473
1060.397729	66.882277	69.038478
1060.144380	62.259526	69.043482
1059.261248	62.133536	69.048487
1058.429734	63.311370	69.053492
1057.405542	57.669516	69.058497
1057.403741	68.823718	69.063502
1056.948682	59.888513	69.068506
1055.926722	57.714052	69.073511
1055.133012	53.196184	69.078516
1054.152014	61.648684	69.083521
1053.779920	64.290980	69.088526
1053.600405	60.238386	69.093530
1052.612575	70.983308	69.098535
1051.776368	56.351234	69.103540
1050.964273	68.545817	69.108545
1050.843969	58.633261	69.113550
1050.497264	61.949614	69.118554
1049.081206	64.442585	69.123559
1048.735609	58.632863	69.128564
1048.002326	69.447682	69.133569
1047.370334	61.573537	69.138574
1046.447090	68.310578	69.143578
1045.855963	64.364463	69.148583
1045.602082	56.860684	69.153588
1045.060857	63.019709	69.158593
1044.182309	50.502783	69.163598
1043.068353	51.843823	69.168602
1042.363867	52.608791	69.173607
1042.128599	52.936415	69.178612
1041.705004	59.131921	69.183617
1040.517949	54.500010	69.188622
1040.087241	56.574462	69.193626
1039.263698	67.584990	69.198631
1039.278413	52.470629	69.203636
1037.916873	53.267581	69.208641
1037.120290	56.985085	69.213646
1036.508469	48.432801	69.218650
1036.121907	50.709966	69.223655
1036.140273	56.147608	69.228660
1035.064471	56.290398	69.233665
1034.924076	54.483490	69.238670
1033.945180	47.544489	69.243674
1032.566998	64.941642	69.248679
1032.612685	48.855680	69.253684
1031.173378	63.248979	69.258689
1030.220462	66.045178	69.263694
1030.110420	59.243923	69.268698
1028.996695	58.542764	69.273703
1028.630337	53.215748	69.278708
1027.880159	53.768790	69.283713
1027.440554	58.825122	69.288718
1027.245422	61.100222	69.293722
1025.726106	61.427113	69.298727
1025.273155	47.591959	69.303732
1024.483331	61.669047	69.308737
1024.448782	54.751705	69.313742
1024.044801	56.148544	69.318746
1023.023815	59.073846	69.323751
1022.352649	51.111328	69.328756
1021.584621	53.923848	69.333761
1021.040154	49.609195	69.338766
1019.957595	56.440970	69.343770
1019.340555	53.426242	69.348775
1018.858973	53.819862	69.353780
1018.204557	60.250788	69.358785
1017.771517	54.786148	69.363790
1017.138870	54.942024	69.368794
1016.294802	57.512751	69.373799
1016.143775	48.869820	69.378804
1014.915040	53.077129	69.383809
1014.167301	42.597352	69.388814
1013.675590	48.428375	69.393818
1013.443097	58.906477	69.398823
1012.587341	48.793966	69.403828
1011.466375	46.236305	69.408833
1010.807053	50.218986	69.413838
1010.334937	57.425162	69.418842
1009.293230	47.810595	69.423847
1008.729555	47.215905	69.428852
1008.146114	52.356621	69.433857
1007.578058	43.504072	69.438862
1007.431177	49.083117	69.443866
1006.648132	51.177356	69.448871
1005.766968	55.411376	69.453876
1004.651086	55.167891	69.458881
1004.517970	57.901484	69.463886
1004.068961	64.277659	69.468890
1002.773748	60.095061	69.473895
1002.514523	54.601195	69.478900
1001.915567	59.695497	69.483905
1001.445880	60.161345	69.488910
1000.454163	61.208565	69.493914
999.302922	62.449901	69.498919
999.274416	51.354223	69.503924
998.664576	52.471577	69.508929
997.800131	50.074962	69.513934
997.028184	48.474191	69.518938
996.056421	48.515289	69.523943
995.983891	45.142702	69.528948
995.528745	58.997811	69.533953
994.673128	54.429889	69.538958
993.925867	46.495261	69.543962
993.183986	50.281344	69.548967
992.449749	49.321130	69.553972
991.297317	58.674558	69.558977
990.653119	50.439678	69.563982
990.546740	56.762917	69.568986
989.922853	52.523986	69.573991
989.681949	38.554191	69.578996
988.815787	49.398030	69.584001
987.791240	53.140777	69.589006
987.509606	52.464949	69.594010
986.384556	52.675519	69.599015
985.396127	50.765416	69.604020
984.835815	58.256864	69.609025
983.934117	46.008584	69.614030
983.916018	52.054422	69.619034
983.537232	58.288536	69.624039
983.388888	54.327187	69.629044
982.320214	55.460775	69.634049
981.474103	51.512671	69.639054
980.664262	54.076386	69.644058
979.473736	54.250067	69.649063
979.122288	56.329264	69.654068
978.676919	61.038011	69.659073
978.148395	50.204819	69.664078
977.656433	54.124610	69.669082
976.441634	63.801785	69.674087
976.030165	55.646575	69.679092
975.247911	63.636967	69.684097
974.540633	57.356522	69.689102
973.809882	56.228600	69.694106
972.955317	61.444002	69.699111
972.405987	57.338292	69.704116
972.162197	57.720895	69.709121
971.693342	60.181475	69.714126
971.040107	57.087363	69.719130
970.048312	61.682775	69.724135
969.897906	48.452366	69.729140
969.117688	62.721901	69.734145
968.186877	55.633349	69.739150
967.848566	53.988824	69.744154
966.515788	58.816686	69.749159
965.961958	63.429151	69.754164
964.896444	65.563616	69.759169
964.425705	59.742282	69.764174
964.045500	54.551524	69.769178
963.633758	62.385195	69.774183
963.403976	50.255520	69.779188
961.897689	56.102900	69.784193
961.374578	55.785620	69.789198
961.165291	52.955191	69.794202
959.931261	62.813628	69.799207
959.152519	59.413056	69.804212
958.323508	64.528203	69.809217
957.952179	57.085705	69.814222
958.058448	52.214941	69.819226
957.191889	58.990294	69.824231
956.181712	54.344477	69.829236
955.607375	59.677723	69.834241
955.259784	54.762477	69.839246
954.470764	57.663512	69.844250
953.105148	61.542543	69.849255
952.812061	51.638576	69.854260
952.394548	54.609810	69.859265
951.631988	57.787334	69.864270
950.577839	53.418177	69.869274
950.172107	57.171287	69.874279
949.593186	50.245954	69.879284
949.235486	65.014395	69.884289
948.309350	62.837348	69.889294
947.732480	54.678501	69.894298
946.835511	59.216255	69.899303
946.714032	57.434729	69.904308
945.599474	59.002990	69.909313
944.734896	56.067093	69.914318
944.414029	53.525658	69.919322
943.359333	48.205684	69.924327
942.485074	54.373557	69.929332
941.904775	54.549508	69.934337
941.459418	49.490550	69.939342
941.124014	47.884991	69.944346
940.706750	52.393724	69.949351
940.188042	56.697825	69.954356
939.083152	59.833629	69.959361
938.443604	61.056650	69.964366
937.610435	52.178493	69.969370
936.672860	51.936629	69.974375
936.023715	50.341568	69.979380
935.490396	58.191430	69.984385
935.048776	59.912818	69.989390
934.850660	59.455520	69.994394
934.060411	63.771292	69.999399
933.070497	57.226750	70.004404
932.188098	61.552455	70.009409
931.878517	59.950671	70.014414
930.964790	59.626166	70.019418
929.658016	56.613980	70.024423
929.412110	56.591644	70.029428
928.830537	56.299443	70.034433
928.307201	60.235274	70.039438
928.334225	56.253910	70.044442
927.373219	61.199255	70.049447
926.557346	51.037857	70.054452
926.091233	57.024095	70.059457
925.407810	62.139738	70.064462
924.694895	57.339399	70.069466
923.914854	61.169421	70.074471
923.539976	57.384475	70.079476
922.260629	63.806052	70.084481
921.350282	66.521397	70.089486
921.198378	61.850986	70.094490
920.476699	66.638402	70.099495
920.212735	54.288667	70.104500
919.061091	68.314542	70.109505
918.462104	60.963471	70.114510
918.121594	46.082283	70.119514
917.322284	60.548828	70.124519
916.469107	49.291074	70.129524
915.757668	55.973944	70.134529
914.918724	60.396818	70.139534
914.990897	59.980091	70.144538
913.791591	58.176112	70.149543
912.834499	53.621216	70.154548
912.268481	59.648586	70.159553
911.687844	58.045784	70.164558
911.673076	57.193457	70.169562
910.947936	63.577311	70.174567
909.761930	50.980064	70.179572
908.993979	54.612622	70.184577
908.514833	64.302070	70.189582
908.360204	58.818381	70.194586
907.896748	68.935846	70.199591
906.996640	56.280485	70.204596
906.329722	66.312053	70.209601
905.183890	63.017223	70.214606
904.353905	59.545976	70.219610
903.733268	70.205699	70.224615
903.371824	58.557455	70.229620
903.138702	62.191641	70.234625
901.762334	57.687699	70.239630
901.482575	53.813504	70.244634
900.595513	62.404065	70.249639
900.172131	54.651319	70.254644
899.202824	60.060044	70.259649
898.104376	58.891308	70.264654
897.795942	63.732817	70.269658
897.329730	62.567551	70.274663
897.285613	53.450304	70.279668
896.497797	55.023361	70.284673
895.381381	54.433078	70.289678
895.115581	52.384361	70.294682
894.315171	64.372105	70.299687
893.429048	50.516039	70.304692
892.514403	56.926897	70.309697
891.920822	63.895374	70.314702
891.815259	54.202853	70.319706
890.517507	70.339886	70.324711
889.675337	61.267633	70.329716
889.428839	61.630174	70.334721
888.975488	65.837153	70.339726
888.616588	61.559233	70.344730
887.216890	72.148970	70.349735
886.565936	53.794251	70.354740
886.214620	55.405079	70.359745
885.367532	61.890347	70.364750
885.042724	55.602686	70.369754
883.944894	61.110716	70.374759
883.288258	55.728999	70.379764
882.967794	62.718668	70.384769
882.275441	62.453568	70.389774
882.173563	55.874962	70.394778
881.036308	59.116865	70.399783
880.532332	50.120114	70.404788
879.406860	54.760483	70.409793
878.790097	56.615408	70.414798
878.453835	59.641531	70.419802
877.603565	60.472322	70.424807
877.171268	56.409515	70.429812
876.141301	61.542470	70.434817
875.278075	64.035865	70.439822
874.689337	50.129328	70.444826
874.195200	60.377829	70.449831
873.681578	54.867698	70.454836
872.947455	57.791558	70.459841
872.112669	56.304906	70.464846
871.669018	61.407633	70.469850
871.037277	56.854593	70.474855
870.654862	51.058654	70.479860
869.581535	58.691688	70.484865
868.520530	58.210870	70.489870
868.825660	49.675141	70.494874
867.683209	56.612696	70.499879
866.575474	56.246549	70.504884
866.277814	52.931876	70.509889
865.822151	62.616012	70.514894
865.662371	54.466507	70.519898
864.242564	64.859175	70.524903
863.591772	56.347840	70.529908
863.063667	54.854962	70.534913
862.481650	58.757565	70.539918
861.993332	51.570255	70.544922
860.744847	64.807306	70.549927
860.245266	51.746028	70.554932
860.077397	53.381281	70.559937
858.890733	55.468836	70.564942
858.417036	54.678510	70.569946
857.698946	53.900270	70.574951
857.217731	62.025704	70.579956
856.826954	59.656258	70.584961
855.706160	57.499189	70.589966
855.199815	57.193456	70.594970
854.497527	62.267961	70.599975
854.328766	55.961778	70.604980
852.735087	48.393725	70.609985
852.473233	60.336762	70.614990
851.966228	45.545171	70.619994
851.228038	52.943519	70.624999
850.367342	56.180843	70.630004
849.550750	57.722223	70.635009
848.901199	55.499620	70.640014
848.746478	47.156928	70.645018
848.199628	59.886494	70.650023
847.464227	55.646428	70.655028
846.338906	48.680355	70.660033
845.768397	55.097957	70.665038
845.471741	44.748307	70.670042
844.231828	53.905971	70.675047
843.563150	48.450491	70.680052
843.253327	49.997951	70.685057
842.530309	56.804105	70.690062
842.630485	41.190483	70.695066
841.242575	56.324728	70.700071
840.630103	60.616961	70.705076
840.289471	51.797651	70.710081
838.804139	56.436964	70.715086
838.207659	56.979792	70.720090
837.709051	59.932409	70.725095
837.409835	59.070162	70.730100
837.007857	57.632909	70.735105
836.000230	54.172616	70.740110
835.453289	55.951782	70.745114
834.559796	60.038006	70.750119
834.029445	58.394103	70.755124
833.539154	56.830558	70.760129
832.388926	54.287099	70.765134
832.005996	56.875951	70.770138
831.500142	55.958283	70.775143
830.961054	49.588045	70.780148
830.093064	54.143298	70.785153
828.921820	61.161146	70.790158
828.769601	57.744481	70.795162
828.286210	67.458267	70.800167
827.395200	54.210139	70.805172
826.851964	46.706729	70.810177
825.755912	48.355673	70.815182
825.758652	49.514339	70.820186
824.366091	52.106191	70.825191
823.917737	57.744261	70.830196
823.497297	48.373108	70.835201
822.898258	51.652372	70.840206
822.554841	50.221572	70.845210
821.438980	49.071413	70.850215
820.708140	45.578112	70.855220
820.439903	39.379238	70.860225
819.303559	52.547980	70.865230
818.591638	45.210194	70.870234
817.664613	54.382724	70.875239
817.323227	43.693269	70.880244
817.259169	43.750811	70.885249
816.384845	42.532248	70.890254
815.606996	47.060540	70.895258
814.456950	55.628323	70.900263
813.956368	56.740945	70.905268
813.880673	60.171881	70.910273
812.894132	55.400941	70.915278
812.241519	52.497589	70.920282
811.585868	47.382247	70.925287
811.075069	45.389885	70.930292
810.327006	43.894183	70.935297
809.411078	53.697309	70.940302
809.249407	46.033822	70.945306
808.130237	45.719985	70.950311
806.951373	52.161883	70.955316
806.531975	50.591791	70.960321
806.234672	53.133901	70.965326
805.716912	44.358567	70.970330
805.357826	54.953005	70.975335
804.494025	47.823902	70.980340
803.646912	43.319360	70.985345
803.185700	52.419325	70.990350
802.438044	45.412087	70.995354
801.447039	48.767937	71.000359
800.635130	51.089181	71.005364
800.350076	45.011257	71.010369
799.832271	50.597303	71.015374
798.907944	50.910048	71.020378
798.012465	54.641782	71.025383
797.716292	51.159726	71.030388
797.185799	40.025715	71.035393
796.259200	46.908434	71.040398
795.476796	51.689771	71.045402
794.783486	50.437672	71.050407
794.220623	46.829332	71.055412
794.008232	46.607709	71.060417
793.336061	44.335107	71.065422
792.258557	44.320575	71.070426
791.702566	53.254278	71.075431
791.456206	40.032879	71.080436
790.692944	48.088089	71.085441
789.691711	50.950408	71.090446
789.264166	45.065478	71.095450
788.436740	50.547845	71.100455
787.396486	53.663958	71.105460
786.964876	47.129968	71.110465
786.330604	55.678740	71.115470
786.223846	46.065278	71.120474
785.445455	46.711191	71.125479
784.475023	45.736597	71.130484
783.822015	54.174810	71.135489
783.287325	55.680799	71.140494
782.422090	45.975182	71.145498
781.684154	51.687735	71.150503
780.829906	43.948417	71.155508
780.447380	42.421347	71.160513
779.790283	43.445348	71.165518
779.403931	38.422770	71.170522
778.103976	42.121121	71.175527
777.712222	53.968133	71.180532
777.184796	49.463174	71.185537
776.632143	51.571269	71.190542
775.912663	51.061358	71.195546
775.277699	47.097069	71.200551
774.767027	56.274298	71.205556
774.241340	51.010544	71.210561
773.210350	50.170174	71.215566
772.438513	37.898180	71.220570
771.857765	52.229023	71.225575
771.520261	50.089234	71.230580
770.434234	49.609288	71.235585
769.343778	52.132578	71.240590
769.057765	40.787770	71.245594
768.554671	45.955160	71.250599
768.202305	43.412460	71.255604
767.400030	47.548837	71.260609
766.592325	50.001886	71.265614
766.050400	45.835132	71.270618
765.542551	43.966890	71.275623
764.457848	53.328537	71.280628
764.048579	42.186277	71.285633
763.148454	52.677606	71.290638
763.022569	45.421593	71.295642
761.829637	45.868574	71.300647
761.070710	48.222397	71.305652
760.799296	47.015111	71.310657
759.924181	50.015059	71.315662
759.495934	47.194280	71.320666
758.376074	47.295315	71.325671
757.806272	53.187690	71.330676
757.559012	46.381509	71.335681
756.787400	51.875500	71.340686
756.666695	40.499650	71.345690
755.607075	46.668694	71.350695
754.511349	48.677162	71.355700
754.394194	47.420090	71.360705
753.188587	59.127005	71.365710
752.618742	43.424511	71.370714
751.829259	53.106597	71.375719
751.097722	55.566450	71.380724
751.459025	43.964054	71.385729
750.071415	50.721481	71.390734
749.802051	46.440378	71.395738
748.985687	43.577307	71.400743
747.965322	49.853647	71.405748
747.168090	43.428335	71.410753
746.291183	48.033916	71.415758
746.165103	46.056018	71.420762
745.732667	50.265989	71.425767
745.223586	49.758863	71.430772
744.456596	44.016292	71.435777
743.715050	49.924970	71.440782
743.051325	53.200356	71.445786
742.279887	48.636481	71.450791
741.299305	57.303470	71.455796
741.261086	47.392096	71.460801
739.926716	56.679958	71.465806
739.188052	43.385554	71.470810
738.654058	52.774656	71.475815
738.107482	53.964001	71.480820
738.059666	53.017589	71.485825
736.838435	57.007784	71.490830
736.051668	52.794857	71.495834
735.284430	56.181342	71.500839
734.766969	59.133824	71.505844
734.620280	56.793352	71.510849
733.797884	59.486872	71.515854
733.185131	50.668331	71.520858
732.536865	52.905197	71.525863
731.319967	58.460625	71.530868
730.735674	59.831018	71.535873
729.693961	57.139445	71.540878
729.330023	58.026902	71.545882
728.771689	54.778980	71.550887
728.581712	54.831339	71.555892
728.219299	49.076403	71.560897
727.051702	60.545464	71.565902
726.270908	46.127090	71.570906
726.056400	51.750018	71.575911
724.948664	50.004096	71.580916
724.063604	51.065980	71.585921
723.628822	55.216405	71.590926
723.373548	47.635641	71.595930
722.550408	52.177477	71.600935
721.550692	49.769384	71.605940
721.016561	50.794324	71.610945
720.548826	52.220279	71.615950
720.084851	46.713328	71.620954
719.140262	54.368492	71.625959
718.375111	51.636049	71.630964
718.206539	50.259431	71.635969
717.067726	58.517956	71.640974
716.106872	51.814349	71.645978
715.780556	47.181194	71.650983
714.993005	53.012049	71.655988
714.764179	51.853182	71.660993
713.383197	50.984979	71.665998
713.022164	50.635640	71.671002
712.369724	48.186454	71.676007
711.784757	55.036889	71.681012
711.688006	50.181104	71.686017
710.280728	57.602430	71.691022
710.076347	43.581154	71.696026
709.597657	39.976784	71.701031
707.854245	53.015130	71.706036
707.624749	48.552643	71.711041
706.660702	57.939257	71.716046
706.282222	53.073132	71.721050
706.184708	45.041478	71.726055
705.435568	52.235018	71.731060
704.456531	47.803557	71.736065
703.799644	63.925347	71.741070
703.320889	49.920941	71.746074
702.866619	51.480374	71.751079
701.540945	60.542943	71.756084
701.320049	52.359040	71.761089
700.570510	52.144097	71.766094
700.202419	53.245108	71.771098
698.910267	58.020898	71.776103
698.243542	63.067698	71.781108
698.267262	52.260214	71.786113
697.747574	51.981869	71.791118
697.014168	50.892301	71.796122
696.018523	56.226435	71.801127
695.272542	64.293116	71.806132
694.737673	61.013080	71.811137
693.669873	62.329576	71.816142
692.892028	60.460181	71.821146
692.644676	59.548694	71.826151
691.924917	57.647974	71.831156
691.857124	50.444220	71.836161
690.616289	57.498432	71.841166
689.939326	52.101091	71.846170
689.808474	49.378055	71.851175
688.699811	60.009843	71.856180
687.873670	45.250200	71.861185
687.321107	55.195778	71.866190
686.933431	55.672279	71.871194
685.796019	51.046844	71.876199
684.883476	56.962264	71.881204
684.559247	46.183377	71.886209
683.707118	53.494246	71.891214
683.423040	56.838510	71.896218
683.471266	57.215647	71.901223
682.107069	58.645571	71.906228
681.652962	50.153451	71.911233
680.842339	60.884445	71.916238
680.193380	62.684617	71.921242
679.251892	47.470254	71.926247
678.655128	48.248131	71.931252
678.292638	49.006053	71.936257
677.641814	55.507432	71.941262
676.530964	46.681489	71.946266
676.017209	53.643593	71.951271
675.374125	56.486776	71.956276
675.195880	39.493516	71.961281
674.129395	44.001568	71.966286
673.250678	47.716479	71.971290
672.826985	48.313835	71.976295
672.016772	56.024889	71.981300
671.685450	55.420089	71.986305
670.350233	57.094564	71.991310
669.813208	39.267451	71.996314
669.433308	55.289937	72.001319
668.925033	55.225824	72.006324
668.777147	39.322141	72.011329
667.882788	53.780198	72.016334
667.000717	52.726926	72.021338
666.696243	43.670092	72.026343
665.295716	54.562821	72.031348
664.704986	49.386726	72.036353
663.880197	47.665166	72.041358
663.933989	52.605130	72.046362
662.923412	54.292573	72.051367
661.783452	57.546037	72.056372
661.331235	53.106402	72.061377
660.708862	48.827904	72.066382
660.489424	46.588910	72.071386
660.091840	49.184846	72.076391
659.213313	53.984679	72.081396
658.493654	44.147129	72.086401
657.815075	47.631480	72.091406
657.018285	50.000822	72.096410
656.095310	50.952072	72.101415
655.315427	55.589542	72.106420
655.075527	44.729427	72.111425
654.607891	61.207438	72.116430
653.441974	46.296909	72.121434
652.892663	52.141884	72.126439
652.382534	52.503847	72.131444
652.120538	44.164076	72.136449
650.682714	57.292570	72.141454
650.113495	53.680548	72.146458
649.843134	45.635422	72.151463
649.522436	46.974898	72.156468
648.949857	49.081459	72.161473
648.095069	51.463193	72.166478
647.272651	53.732540	72.171482
646.214351	57.931798	72.176487
644.890136	53.840754	72.181492
644.844514	45.903346	72.186497
644.175875	56.103956	72.191502
644.006764	55.681488	72.196506
643.778688	57.900352	72.201511
642.343471	57.302599	72.206516
642.199423	46.157563	72.211521
641.213566	56.457572	72.216526
640.195989	55.998322	72.221530
639.729844	43.045345	72.226535
638.986065	52.568788	72.231540
638.707861	50.247690	72.236545
638.201919	59.826306	72.241550
637.158829	46.041101	72.246554
636.486601	51.208636	72.251559
635.816761	50.903751	72.256564
635.349237	45.637083	72.261569
633.988653	50.365450	72.266574
633.454804	50.857351	72.271578
632.951634	50.691507	72.276583
632.474742	52.822258	72.281588
632.283131	42.545819	72.286593
631.243391	46.664853	72.291598
630.504856	45.834743	72.296602
630.339970	42.131535	72.301607
629.596696	48.489947	72.306612
628.640782	39.565245	72.311617
627.890575	45.913721	72.316622
627.318744	50.738841	72.321626
626.921201	45.986157	72.326631
625.293700	58.354812	72.331636
624.765653	43.915165	72.336641
624.240184	55.293042	72.341646
624.078397	52.480319	72.346650
624.046497	42.959042	72.351655
622.635164	56.639994	72.356660
621.839385	49.116936	72.361665
621.255212	50.387985	72.366670
620.684480	48.017278	72.371674
619.821076	48.239963	72.376679
618.778220	56.603090	72.381684
618.794868	39.777505	72.386689
618.263356	47.343261	72.391694
617.897812	47.396778	72.396698
617.127922	43.411446	72.401703
615.897451	53.736220	72.406708
615.517790	42.991412	72.411713
614.415819	50.575473	72.416718
613.587759	49.934667	72.421722
613.226315	48.748044	72.426727
612.693419	53.489696	72.431732
612.703264	48.210091	72.436737
611.485995	54.069980	72.441742
610.569130	51.798551	72.446746
610.247088	44.788262	72.451751
609.568743	51.372883	72.456756
608.910727	57.498530	72.461761
607.720905	52.159233	72.466766
607.149295	46.249980	72.471770
606.743247	51.378286	72.476775
606.331671	46.929040	72.481780
605.899204	40.704318	72.486785
604.729702	47.334039	72.491790
604.285863	50.298471	72.496794
603.437028	47.795438	72.501799
602.421606	53.782459	72.506804
602.131466	46.133154	72.511809
601.555375	51.383158	72.516814
601.067970	43.604420	72.521818
600.488800	50.431869	72.526823
599.400914	54.191153	72.531828
599.189450	49.304762	72.536833
598.361609	48.471538	72.541838
597.121588	54.327171	72.546842
596.596030	54.235863	72.551847
595.902823	47.535421	72.556852
595.794412	43.140401	72.561857
595.398359	48.032149	72.566862
594.132790	50.542397	72.571866
593.624510	54.004374	72.576871
593.004946	58.318285	72.581876
592.508611	44.925428	72.586881
590.964880	52.937821	72.591886
590.625214	52.891026	72.596890
590.203042	45.999190	72.601895
589.594119	62.688938	72.606900
589.469810	52.676172	72.611905
588.311986	64.109034	72.616910
587.477088	46.829279	72.621914
587.105964	41.842163	72.626919
586.298574	50.987815	72.631924
585.763653	42.861834	72.636929
584.757422	48.118841	72.641934
584.608466	45.125885	72.646938
584.010171	50.082959	72.651943
582.944635	56.077968	72.656948
582.370584	45.359395	72.661953
581.993014	53.873623	72.666958
581.003839	48.186997	72.671962
579.868140	49.107497	72.676967
579.275813	51.244026	72.681972
579.198961	43.000940	72.686977
578.739105	47.454996	72.691982
577.913382	47.312148	72.696986
577.080681	39.181557	72.701991
576.297366	47.219506	72.706996
576.030643	41.315324	72.712001
574.952587	39.758712	72.717006
573.954829	47.154301	72.722010
573.878824	42.583810	72.727015
573.226911	44.673059	72.732020
572.732147	42.009569	72.737025
571.714707	48.301271	72.742030
570.553411	47.270428	72.747034
570.495033	44.468051	72.752039
570.034700	54.022059	72.757044
569.428108	44.412543	72.762049
568.232929	46.471621	72.767054
567.472187	49.475492	72.772058
567.455148	47.171157	72.777063
566.810249	52.294930	72.782068
565.671003	48.865182	72.787073
565.155939	49.767267	72.792078
564.526931	56.825014	72.797082
564.136388	44.839309	72.802087
562.555064	55.827112	72.807092
562.269187	48.039941	72.812097
561.455811	54.715465	72.817102
561.411049	49.236402	72.822106
561.262439	53.185150	72.827111
560.048443	64.677431	72.832116
559.739904	52.861588	72.837121
558.597048	58.085174	72.842126
557.202617	65.116600	72.847130
556.983334	52.993228	72.852135
556.243357	58.666736	72.857140
556.345231	43.292578	72.862145
555.782782	54.155954	72.867150
554.289198	49.317654	72.872154
553.734025	41.742113	72.877159
552.828841	48.351834	72.882164
553.125567	39.752786	72.887169
552.288893	45.916355	72.892174
551.079022	47.564619	72.897178
550.658341	38.600439	72.902183
550.162640	54.190357	72.907188
549.441586	46.101916	72.912193
548.220860	48.144572	72.917198
547.526572	44.074683	72.922202
547.466684	41.099083	72.927207
547.026823	50.692408	72.932212
546.050022	48.299664	72.937217
545.119400	45.879065	72.942222
544.501023	48.724649	72.947226
544.201511	44.945121	72.952231
543.835007	49.846361	72.957236
542.746929	37.249524	72.962241
541.921676	46.006943	72.967246
541.331912	42.650538	72.972250
541.291769	44.416850	72.977255
540.158473	49.001828	72.982260
539.325758	42.479748	72.987265
538.813238	45.246971	72.992270
537.475207	48.811154	72.997274
536.828321	49.732665	73.002279
536.288873	52.472639	73.007284
535.959761	46.542129	73.012289
535.880367	47.139862	73.017294
534.997054	56.061078	73.022298
534.644859	36.223929	73.027303
533.390322	51.332313	73.032308
533.069671	48.680522	73.037313
532.483106	57.860403	73.042318
531.022731	52.592627	73.047322
530.501826	55.736504	73.052327
529.966029	52.365196	73.057332
529.570301	43.438046	73.062337
529.147880	48.967936	73.067342
528.115668	55.236778	73.072346
527.810811	48.472927	73.077351
527.050648	54.651128	73.082356
526.083903	50.851723	73.087361
524.999754	51.697804	73.092366
524.607323	54.504251	73.097370
524.508762	58.165908	73.102375
523.709246	56.553911	73.107380
523.250378	44.941802	73.112385
521.999294	54.975006	73.117390
521.207687	52.540157	73.122394
521.051836	52.675406	73.127399
520.426879	50.805371	73.132404
519.455588	50.252066	73.137409
518.830514	46.097045	73.142414
518.142716	50.980079	73.147418
518.000866	44.756393	73.152423
516.952744	46.796802	73.157428
516.240645	48.917729	73.162433
515.807065	46.670283	73.167438
515.042554	50.874831	73.172442
514.756278	40.750690	73.177447
513.618573	49.255112	73.182452
513.279087	44.277163	73.187457
512.393495	57.489641	73.192462
511.359032	51.892261	73.197466
510.988858	45.162473	73.202471
510.069092	54.494778	73.207476
509.966393	55.780622	73.212481
509.192323	46.059031	73.217486
508.259996	50.932133	73.222490
507.976431	47.858122	73.227495
507.114103	58.043875	73.232500
506.187670	52.771488	73.237505
505.458458	49.353726	73.242510
504.615384	50.806390	73.247514
504.727813	40.421622	73.252519
504.028371	49.444440	73.257524
503.086832	45.439181	73.262529
502.206349	48.534683	73.267534
501.698195	54.176007	73.272538
501.573571	39.818804	73.277543
500.500488	40.278357	73.282548
499.424531	45.104952	73.287553
499.197415	46.230842	73.292558
498.332117	49.864822	73.297562
498.115920	50.534810	73.302567
496.789638	51.127738	73.307572
496.274235	43.038099	73.312577
496.049330	40.823649	73.317582
495.289896	50.493115	73.322586
494.411694	41.548213	73.327591
493.452176	48.180799	73.332596
493.122845	45.833173	73.337601
492.814598	40.613710	73.342606
491.948072	53.592916	73.347610
491.421336	43.526006	73.352615
490.609187	47.123136	73.357620
490.103767	44.975449	73.362625
489.065274	48.215974	73.367630
488.267886	50.498728	73.372634
488.029797	49.103241	73.377639
487.418925	53.340093	73.382644
486.492314	51.633238	73.387649
485.657198	45.534184	73.392654
484.942287	49.688261	73.397658
484.844567	51.500016	73.402663
484.360358	50.649937	73.407668
483.322959	47.349085	73.412673
482.628611	43.870584	73.417678
481.780222	43.693532	73.422682
481.702523	42.389190	73.427687
480.730965	44.513611	73.432692
479.956778	53.158835	73.437697
479.497348	53.758762	73.442702
478.119653	55.826458	73.447706
477.733980	43.027873	73.452711
476.924255	54.208193	73.457716
476.394254	42.992208	73.462721
476.312097	54.014047	73.467726
475.819099	53.537532	73.472730
474.960053	51.015672	73.477735
473.668225	53.555392	73.482740
473.202565	48.782053	73.487745
473.067141	40.316500	73.492750
471.863399	48.583875	73.497754
471.538989	48.755440	73.502759
470.531500	47.908300	73.507764
470.355502	47.113205	73.512769
469.550893	46.896066	73.517774
468.443228	53.128062	73.522778
468.233049	42.897190	73.527783
467.685004	44.228750	73.532788
466.756390	48.232371	73.537793
465.824548	46.624129	73.542798
465.174143	49.679837	73.547802
464.958399	53.453201	73.552807
464.400932	51.145075	73.557812
463.146446	50.446097	73.562817
462.481832	54.022887	73.567822
461.920740	55.985732	73.572826
461.734950	47.160770	73.577831
460.879299	50.141943	73.582836
459.712054	45.327412	73.587841
459.355426	44.263049	73.592846
458.937263	46.143199	73.597850
458.815637	39.056862	73.602855
457.541967	50.186514	73.607860
456.740769	49.863181	73.612865
456.517126	47.689534	73.617870
455.479461	61.194336	73.622874
454.672925	50.424531	73.627879
453.803574	55.677127	73.632884
453.294841	51.954597	73.637889
453.171999	51.666698	73.642894
452.480126	49.618108	73.647898
451.511385	44.078099	73.652903
450.993447	54.934396	73.657908
450.446087	50.385389	73.662913
449.851109	45.017647	73.667918
448.829961	52.741857	73.672922
448.292793	42.041112	73.677927
448.092397	51.045937	73.682932
447.182780	48.112675	73.687937
446.166063	46.680389	73.692942
445.690686	50.588157	73.697946
444.942123	46.063323	73.702951
443.675420	49.305530	73.707956
442.972195	53.399409	73.712961
442.986439	48.245269	73.717966
441.919987	53.578154	73.722970
441.644570	47.645415	73.727975
441.491067	53.635522	73.732980
440.812335	55.263876	73.737985
440.095403	54.796235	73.742990
439.010217	54.538652	73.747994
437.739377	46.816964	73.752999
437.376432	50.465547	73.758004
436.827604	54.407096	73.763009
436.458662	42.411682	73.768014
436.036410	60.484646	73.773018
435.567397	43.674963	73.778023
434.547788	51.701707	73.783028
433.693634	55.766018	73.788033
432.908697	47.711453	73.793038
431.883206	48.605000	73.798042
431.547577	49.841224	73.803047
430.819012	48.523885	73.808052
430.422988	42.342284	73.813057
430.380449	46.550100	73.818062
429.132076	46.957186	73.823066
428.499455	45.591446	73.828071
428.094238	47.165186	73.833076
427.116548	44.318472	73.838081
426.339297	45.699173	73.843086
425.501600	51.492358	73.848090
425.473489	41.880615	73.853095
424.878549	48.368405	73.858100
423.925920	40.972922	73.863105
423.331434	53.583949	73.868110
422.770190	56.021489	73.873114
421.695160	47.385519	73.878119
420.859023	52.093513	73.883124
420.702719	41.959724	73.888129
420.382350	50.412807	73.893134
419.042726	45.778725	73.898138
418.234646	53.752850	73.903143
417.703061	61.980972	73.908148
417.316363	46.055466	73.913153
416.718593	49.465497	73.918158
415.412483	51.605399	73.923162
414.756802	50.035179	73.928167
414.244797	47.782901	73.933172
413.923305	46.831219	73.938177
414.006117	48.448630	73.943182
412.918704	57.443398	73.948186
412.116335	49.399502	73.953191
411.850286	55.950014	73.958196
410.451115	54.496676	73.963201
409.920186	53.739212	73.968206
408.786954	62.348623	73.973210
408.701885	53.728392	73.978215
408.248387	46.940939	73.983220
406.953538	48.833046	73.988225
406.163120	49.936730	73.993230
405.544206	61.965031	73.998234
405.635304	44.219293	74.003239
405.031814	47.101959	74.008244
404.117935	50.444087	74.013249
403.256884	47.935189	74.018254
402.652224	55.697136	74.023258
402.199937	54.523443	74.028263
401.200821	46.094586	74.033268
400.322072	52.503022	74.038273
400.363069	53.173040	74.043278
399.486101	61.218074	74.048282
399.100658	42.234665	74.053287
398.181024	48.174952	74.058292
397.387100	47.869402	74.063297
397.064940	47.990156	74.068302
395.509529	43.650669	74.073306
395.184707	42.248511	74.078311
394.978629	45.141974	74.083316
394.335663	46.709446	74.088321
393.253759	44.503824	74.093326
392.280946	52.575166	74.098330
391.981501	48.585916	74.103335
391.458765	56.541392	74.108340
391.200864	49.569812	74.113345
390.154494	44.248780	74.118350
389.157206	53.585584	74.123354
388.790418	45.942228	74.128359
388.289346	56.324336	74.133364
387.655121	52.114039	74.138369
386.941472	45.860053	74.143374
386.207249	57.804224	74.148378
386.060497	42.531205	74.153383
384.892588	53.295530	74.158388
384.037370	57.587108	74.163393
383.561652	49.978454	74.168398
382.799778	56.250002	74.173402
382.445654	50.462279	74.178407
381.399904	51.103607	74.183412
380.854431	50.302736	74.188417
380.570933	45.060425	74.193422
379.378315	56.866326	74.198426
378.686394	51.752169	74.203431
378.129117	52.782444	74.208436
377.899961	51.125348	74.213441
377.533313	44.554300	74.218446
375.755990	57.860012	74.223450
375.634081	43.284780	74.228455
375.058622	55.195769	74.233460
374.025847	57.896111	74.238465
373.362106	49.681908	74.243470
372.487767	52.770166	74.248474
372.143000	48.296132	74.253479
371.921332	46.434418	74.258484
371.489005	52.874230	74.263489
370.634975	47.457902	74.268494
369.384619	59.733479	74.273498
368.870789	47.526201	74.278503
368.696403	53.759332	74.283508
367.334526	47.769494	74.288513
367.087809	45.553803	74.293518
366.215138	53.591849	74.298522
365.693243	53.623009	74.303527
365.373023	51.537301	74.308532
363.911808	52.732119	74.313537
363.501449	47.555756	74.318542
363.148530	53.613909	74.323546
362.837982	49.859822	74.328551
361.749254	50.340851	74.333556
360.696465	47.674865	74.338561
360.358697	47.473259	74.343566
359.782784	52.753238	74.348570
359.605712	40.206880	74.353575
358.355517	45.594303	74.358580
357.529326	43.235987	74.363585
357.279592	42.529921	74.368590
356.519901	48.189268	74.373594
355.789860	39.211359	74.378599
355.321945	48.976324	74.383604
354.370897	52.286545	74.388609
353.833556	48.598562	74.393614
352.666837	50.561742	74.398618
352.101327	42.599979	74.403623
351.815445	37.971490	74.408628
351.213422	49.497202	74.413633
351.307077	39.569599	74.418638
350.013525	47.733062	74.423642
349.325664	44.110067	74.428647
348.351835	51.104526	74.433652
347.066355	55.113017	74.438657
347.131713	43.565660	74.443662
346.268432	49.309326	74.448666
345.952636	48.623250	74.453671
345.874987	49.215979	74.458676
344.730865	41.761162	74.463681
344.144785	48.332708	74.468686
343.456246	56.287803	74.473690
342.655070	45.826281	74.478695
341.546185	49.286238	74.483700
340.727960	50.462183	74.488705
340.730258	48.566357	74.493710
339.895295	56.573172	74.498714
339.613872	59.440800	74.503719
338.436450	46.908773	74.508724
337.723224	60.180555	74.513729
337.585358	41.416337	74.518734
336.578388	49.937837	74.523738
335.480271	49.515203	74.528743
335.248815	45.273856	74.533748
334.509471	45.623525	74.538753
334.371445	40.700240	74.543758
333.796127	45.243691	74.548762
333.170646	44.236384	74.553767
332.474521	36.582451	74.558772
331.202360	45.970956	74.563777
330.505966	41.827357	74.568782
329.724776	41.980270	74.573786
329.379395	41.693149	74.578791
329.099156	40.944639	74.583796
327.963697	50.235670	74.588801
327.594603	42.635275	74.593806
326.589623	43.927718	74.598810
326.303776	37.474695	74.603815
325.221261	45.667614	74.608820
324.249710	43.909639	74.613825
324.440131	41.800909	74.618830
323.569342	49.253615	74.623834
322.882123	46.097304	74.628839
321.948544	42.436207	74.633844
321.470758	50.649452	74.638849
321.167686	46.217670	74.643854
320.223477	37.674452	74.648858
319.499482	42.692606	74.653863
318.959369	40.944725	74.658868
318.018513	42.171759	74.663873
317.337691	49.753465	74.668878
316.315177	48.692742	74.673882
315.853810	45.032085	74.678887
315.682537	45.412654	74.683892
315.198993	49.410052	74.688897
314.652028	48.185233	74.693902
313.303413	44.547704	74.698906
312.615499	41.905594	74.703911
312.504228	47.754927	74.708916
311.489642	50.799323	74.713921
311.026827	45.650256	74.718926
310.202285	47.410689	74.723930
309.617917	49.758896	74.728935
308.547901	46.627325	74.733940
307.534884	57.221915	74.738945
307.554053	39.648511	74.743950
307.044484	52.233399	74.748954
306.727111	41.720023	74.753959
305.554698	49.216073	74.758964
304.721079	47.481854	74.763969
304.363522	44.735057	74.768974
304.039401	35.807597	74.773978
302.998365	44.429150	74.778983
302.086933	46.955639	74.783988
301.293189	44.139587	74.788993
301.172621	36.908023	74.793998
300.303889	42.704608	74.799002
299.331104	40.617258	74.804007
299.205724	33.266615	74.809012
298.469406	47.243813	74.814017
297.869428	33.787163	74.819022
296.583262	42.029893	74.824026
296.060380	45.197779	74.829031
295.933652	47.307472	74.834036
295.501871	45.870336	74.839041
294.730636	37.422566	74.844046
293.519392	52.024239	74.849050
292.996755	38.779187	74.854055
292.654204	38.051652	74.859060
291.275362	45.954343	74.864065
290.915438	43.143271	74.869070
290.424415	47.487215	74.874074
289.995255	49.518954	74.879079
289.241277	44.619724	74.884084
287.956657	49.407118	74.889089
287.638088	39.540489	74.894094
287.108834	52.415520	74.899098
286.538626	48.283362	74.904103
285.751712	46.374550	74.909108
284.931308	45.803599	74.914113
284.610828	35.136187	74.919118
284.096901	44.571021	74.924122
283.104733	42.381110	74.929127
282.370871	51.532458	74.934132
281.710907	46.309164	74.939137
281.526125	44.988782	74.944142
280.138481	45.400794	74.949146
279.380866	43.624509	74.954151
279.032349	37.165715	74.959156
278.342680	43.624471	74.964161
278.295730	40.995330	74.969166
277.522748	48.932354	74.974170
276.485630	43.277166	74.979175
275.926857	42.886868	74.984180
275.404394	36.894191	74.989185
274.610433	43.290722	74.994190
273.683401	47.508620	74.999194
273.250277	43.274194	75.004199
272.923076	45.303876	75.009204
271.607341	48.061971	75.014209
271.146956	41.911165	75.019214
270.261854	50.567803	75.024218
269.816374	46.543503	75.029223
269.899382	40.936870	75.034228
268.742550	40.127810	75.039233
268.017580	29.747226	75.044238
267.389178	39.802698	75.049242
266.505034	42.105653	75.054247
265.690675	42.432606	75.059252
264.905454	52.964091	75.064257
265.164509	44.930854	75.069262
264.544333	45.012392	75.074266
263.223712	46.651636	75.079271
262.404779	42.824057	75.084276
261.324768	50.461516	75.089281
260.999353	53.533280	75.094286
260.579305	55.486301	75.099290
260.375154	45.268700	75.104295
259.751258	43.609881	75.109300
258.605078	57.669768	75.114305
258.599417	45.602307	75.119310
256.841005	47.424873	75.124314
256.312702	41.748520	75.129319
256.242221	43.909173	75.134324
255.896589	43.051246	75.139329
254.757425	48.999760	75.144334
253.737580	49.551858	75.149338
253.173749	43.381275	75.154343
253.144790	48.088391	75.159348
252.307525	52.369260	75.164353
251.257745	43.964325	75.169358
250.411199	47.503929	75.174362
249.932713	39.249210	75.179367
249.704439	43.377815	75.184372
248.616053	44.098534	75.189377
247.995129	31.843727	75.194382
247.170793	47.456065	75.199386
246.824398	47.788858	75.204391
246.764131	30.776916	75.209396
245.413297	48.818098	75.214401
245.119157	42.844226	75.219406
244.376787	49.141081	75.224410
243.727717	40.044654	75.229415
243.204731	39.973512	75.234420
242.314354	50.723610	75.239425
241.665500	38.845411	75.244430
240.578966	43.031972	75.249434
239.842565	50.201507	75.254439
239.791748	46.044920	75.259444
238.954173	49.684023	75.264449
238.119406	46.608028	75.269454
237.329641	46.976802	75.274458
236.593365	45.339055	75.279463
236.476714	44.613366	75.284468
235.784387	48.016429	75.289473
234.990791	43.096726	75.294478
234.165918	49.763126	75.299482
233.742081	37.823832	75.304487
233.307534	37.175624	75.309492
231.784028	45.382099	75.314497
231.367236	41.302774	75.319502
230.905734	45.697214	75.324506
230.509687	44.765327	75.329511
229.679747	41.863607	75.334516
228.737968	44.193108	75.339521
228.003067	44.248788	75.344526
227.830246	40.969512	75.349530
226.960862	47.231423	75.354535
226.757659	35.657509	75.359540
225.719029	53.877595	75.364545
225.242267	36.969888	75.369550
224.612252	39.889935	75.374554
223.769436	46.672736	75.379559
223.341030	41.707441	75.384564
222.343110	48.909205	75.389569
221.559647	36.166228	75.394574
220.550414	45.711562	75.399578
220.067305	54.501254	75.404583
219.695024	42.303008	75.409588
218.872462	46.843315	75.414593
218.703422	39.088056	75.419598
217.609152	42.928931	75.424602
217.033459	48.789216	75.429607
216.466612	38.780832	75.434612
216.038061	42.712707	75.439617
215.301933	45.966639	75.444622
214.135037	50.003597	75.449626
213.630572	49.207266	75.454631
213.446857	36.534267	75.459636
212.465307	40.032324	75.464641
211.605917	41.177025	75.469646
210.930962	41.909127	75.474650
210.746546	48.823520	75.479655
210.262496	41.807603	75.484660
208.690300	50.102279	75.489665
208.187631	44.145885	75.494670
207.995437	45.567429	75.499674
207.475008	39.361557	75.504679
206.376873	43.023281	75.509684
205.488700	40.922481	75.514689
205.316453	39.287873	75.519694
204.974244	49.490126	75.524698
203.891617	45.734566	75.529703
203.180654	40.588816	75.534708
202.531211	47.175217	75.539713
202.015392	48.832854	75.544718
201.597947	49.586987	75.549722
200.387984	42.514904	75.554727
199.974387	47.322759	75.559732
199.439214	54.862348	75.564737
198.411777	49.030611	75.569742
197.722247	55.897797	75.574746
196.903879	46.878834	75.579751
196.724942	54.162939	75.584756
196.309395	54.535148	75.589761
195.445878	47.273797	75.594766
194.469084	47.467397	75.599770
193.630031	43.895363	75.604775
193.681454	46.572745	75.609780
192.737479	52.611594	75.614785
191.507581	45.003377	75.619790
191.175101	52.860737	75.624794
190.632977	54.937308	75.629799
190.542254	38.441155	75.634804
189.330756	41.252060	75.639809
188.906868	41.953605	75.644814
188.389103	42.935043	75.649818
187.308829	43.222413	75.654823
186.546945	40.063856	75.659828
185.853333	39.628844	75.664833
185.525985	37.263606	75.669838
184.896841	42.845411	75.674842
183.598919	48.303600	75.679847
183.189407	38.358455	75.684852
182.229032	49.607002	75.689857
182.170644	55.720717	75.694862
181.626215	49.001435	75.699866
180.899040	48.847741	75.704871
180.376113	45.354624	75.709876
179.654226	54.480430	75.714881
179.015865	48.148284	75.719886
178.262554	55.523958	75.724890
177.432041	57.681200	75.729895
176.922640	49.759430	75.734900
175.412780	51.827857	75.739905
174.848830	47.573307	75.744910
174.518771	49.355875	75.749914
173.760397	55.800380	75.754919
173.607763	51.664759	75.759924
173.110028	58.181254	75.764929
172.866854	56.691994	75.769934
171.742287	48.988147	75.774938
171.038832	57.410853	75.779943
170.738121	48.064946	75.784948
169.045020	53.874727	75.789953
168.549014	42.984587	75.794958
168.046560	45.570499	75.799962
167.584348	48.899046	75.804967
167.297564	40.680019	75.809972
166.042432	50.677736	75.814977
165.776048	41.176552	75.819982
165.138172	46.551597	75.824986
164.294672	51.229300	75.829991
163.225679	42.122578	75.834996
162.726527	49.609119	75.840001
162.244471	47.240162	75.845006
162.035907	36.537591	75.850010
160.741062	42.602423	75.855015
160.223494	39.747122	75.860020
159.416049	49.082111	75.865025
159.181492	41.979123	75.870030
158.386197	39.084523	75.875034
157.502463	40.611590	75.880039
157.565633	39.045109	75.885044
156.535620	40.070375	75.890049
155.142678	50.455919	75.895054
154.822825	41.783275	75.900058
154.213745	44.332572	75.905063
154.070412	39.714504	75.910068
153.316707	45.429715	75.915073
152.520684	54.797581	75.920078
151.996884	39.218882	75.925082
150.844354	45.765653	75.930087
149.937340	40.681140	75.935092
149.238179	46.471235	75.940097
149.050977	40.455102	75.945102
148.941899	43.178571	75.950106
147.882653	44.170654	75.955111
147.122950	45.450871	75.960116
146.273994	43.757002	75.965121
146.055571	44.329602	75.970126
145.041818	41.830957	75.975130
143.806724	45.225961	75.980135
143.623492	36.908430	75.985140
142.973183	42.769584	75.990145
142.395431	39.889190	75.995150
142.385835	41.205931	76.000154
141.253473	38.295692	76.005159
141.002369	32.866913	76.010164
140.051691	47.151123	76.015169
138.916206	42.833168	76.020174
138.242885	39.173231	76.025178
137.459597	41.720345	76.030183
137.382235	42.059145	76.035188
136.906296	41.665134	76.040193
135.561198	36.626823	76.045198
135.152429	38.120747	76.050202
134.256191	44.016383	76.055207
134.078673	35.699520	76.060212
132.743840	44.765363	76.065217
132.311351	43.959151	76.070222
132.045811	32.049847	76.075226
131.152716	45.553749	76.080231
130.908704	34.344330	76.085236
129.846079	43.138115	76.090241
129.338313	44.121125	76.095246
128.972929	41.602688	76.100250
127.971629	43.873906	76.105255
126.981699	41.268969	76.110260
126.248096	48.835473	76.115265
126.011154	50.369812	76.120270
125.577577	42.609436	76.125274
124.446997	53.254361	76.130279
123.940634	53.376135	76.135284
123.330930	49.677672	76.140289
122.579071	54.090041	76.145294
122.189776	42.176810	76.150298
120.966229	56.771044	76.155303
120.680594	40.796414	76.160308
120.182733	50.264976	76.165313
119.539763	48.878894	76.170318
118.559615	51.287093	76.175322
117.777142	46.603779	76.180327
117.631537	44.253727	76.185332
117.145134	53.651079	76.190337
115.800484	50.702159	76.195342
115.562520	45.176668	76.200346
114.806875	54.156483	76.205351
114.406638	46.520101	76.210356
113.033754	48.144102	76.215361
112.399098	46.551693	76.220366
112.205456	40.501898	76.225370
111.713131	49.032872	76.230375
110.689744	43.017609	76.235380
109.985806	57.587344	76.240385
109.722316	51.275870	76.245390
108.957021	51.484666	76.250394
107.884718	51.764491	76.255399
107.533863	51.995514	76.260404
106.712897	46.515675	76.265409
106.189097	44.782590	76.270414
105.513490	39.900894	76.275418
104.639031	46.404922	76.280423
104.412582	38.267753	76.285428
103.593966	42.826385	76.290433
102.423108	45.693928	76.295438
101.771678	39.983635	76.300442
101.092314	46.995872	76.305447
101.435438	44.351849	76.310452
100.469431	47.738661	76.315457
99.494735	47.031527	76.320462
99.231660	41.355503	76.325466
98.285589	52.803644	76.330471
97.472404	50.422847	76.335476
96.808633	44.944756	76.340481
96.000143	52.734520	76.345486
95.515662	44.534415	76.350490
94.905895	52.230991	76.355495
93.956813	47.315633	76.360500
93.503576	52.230746	76.365505
92.667091	54.360582	76.370510
92.370469	41.557376	76.375514
91.889844	54.673827	76.380519
91.025528	47.176107	76.385524
90.274200	57.224410	76.390529
89.567220	42.023447	76.395534
89.072950	38.822251	76.400538
87.945018	55.785592	76.405543
87.891442	36.164339	76.410548
86.937613	45.918498	76.415553
86.714612	49.871231	76.420558
85.663080	42.386022	76.425562
84.628213	52.832772	76.430567
84.239330	46.632764	76.435572
84.088762	45.691719	76.440577
83.111400	47.970177	76.445582
82.250934	42.127643	76.450586
81.283101	54.657891	76.455591
81.421782	41.001532	76.460596
80.194506	50.704683	76.465601
78.989012	50.854373	76.470606
78.830581	37.168126	76.475610
77.949639	42.656063	76.480615
77.801932	41.090092	76.485620
77.590386	43.744748	76.490625
76.582003	52.394289	76.495630
75.734304	45.772286	76.500634
75.166147	53.462230	76.505639
74.781891	41.526132	76.510644
73.352746	42.673427	76.515649
72.860283	42.991690	76.520654
72.627319	44.809249	76.525658
71.931998	47.853285	76.530663
71.164533	46.744111	76.535668
70.517975	52.383912	76.540673
69.688309	50.563992	76.545678
69.274380	46.611977	76.550682
68.255604	53.836043	76.555687
67.491448	44.045250	76.560692
67.150948	44.779250	76.565697
66.680150	49.306083	76.570702
66.343066	43.633982	76.575706
65.221348	47.769455	76.580711
64.503262	38.499598	76.585716
63.858304	46.696949	76.590721
63.042455	46.204195	76.595726
62.439848	45.740513	76.600730
61.622804	47.070900	76.605735
61.274611	44.683773	76.610740
60.691538	38.066888	76.615745
60.310263	51.277881	76.620750
59.524225	45.112828	76.625754
58.733088	50.379873	76.630759
57.723285	45.362252	76.635764
56.744546	46.319459	76.640769
56.099739	46.944293	76.645774
55.971098	46.124332	76.650778
55.201625	43.263497	76.655783
55.199841	45.083614	76.660788
53.989329	35.912792	76.665793
53.028153	42.362853	76.670798
52.842574	35.327769	76.675802
52.048696	44.808849	76.680807
50.908226	40.542197	76.685812
50.476254	50.451266	76.690817
50.103874	44.062555	76.695822
49.944926	37.378036	76.700826
48.433756	44.824131	76.705831
47.845600	47.228190	76.710836
47.197576	45.393504	76.715841
46.709577	47.726398	76.720846
46.315096	45.244154	76.725850
45.260871	54.651643	76.730855
44.974862	48.127732	76.735860
44.316804	52.886283	76.740865
42.941205	52.310915	76.745870
42.546459	53.946121	76.750874
41.657904	56.532130	76.755879
41.372289	51.891031	76.760884
41.004496	47.222037	76.765889
40.449508	43.809763	76.770894
39.759880	40.947238	76.775898
38.741886	49.790710	76.780903
38.203567	50.729726	76.785908
37.274332	42.247332	76.790913
36.552704	47.203677	76.795918
36.243995	43.044078	76.800922
35.609581	60.130581	76.805927
34.736428	43.148962	76.810932
33.931876	44.302324	76.815937
33.301681	46.381932	76.820942
32.949786	48.483388	76.825946
32.140423	54.477167	76.830951
31.198210	45.993690	76.835956
30.693594	47.698458	76.840961
30.125669	51.624202	76.845966
30.228585	42.765890	76.850970
28.707523	47.040760	76.855975
27.985250	44.413679	76.860980
27.654851	41.091746	76.865985
26.787806	38.360022	76.870990
26.220450	41.448316	76.875994
25.015252	46.817675	76.880999
24.697845	46.015206	76.886004
24.395461	52.041670	76.891009
23.730322	47.953110	76.896014
23.138969	41.802755	76.901018
22.178469	47.562019	76.906023
22.113155	38.377305	76.911028
21.576402	50.607003	76.916033
20.872670	43.370708	76.921038
19.928697	41.375074	76.926042
18.702058	53.426221	76.931047
18.432786	52.452073	76.936052
17.673629	51.548171	76.941057
16.917885	52.876680	76.946062
16.293279	52.772908	76.951066
15.749421	53.611888	76.956071
15.207225	45.772669	76.961076
14.148853	48.270653	76.966081
13.232057	55.713438	76.971086
12.752171	47.173579	76.976090
12.264058	51.102366	76.981095
12.266396	50.375058	76.986100
11.161719	49.100490	76.991105
10.095964	57.901131	76.996110
10.164849	51.271738	77.001114
8.904965	54.654992	77.006119
7.817787	47.864631	77.011124
7.224298	49.988854	77.016129
6.953183	53.075637	77.021134
6.442970	42.443281	77.026139
6.119501	53.356909	77.031143
5.337590	51.286546	77.036148
4.194266	51.948327	77.041153
3.610963	54.687512	77.046158