Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3483 bulk_00000.hld	2578.834472	489317.157644	378.015008	144370885.375267	3527.389766	3549.663303	27.874306	3.389306	73.416402	1998.378779	1.198423	-134.399000	-88.703500	0.661454
3483 bulk_00001.hld	2519.536439	496962.933457	358.764536	137664074.874891	3524.647249	3558.441243	27.091561	3.609968	88.949993	1940.856306	1.167757	-134.299000	-88.703500	0.089795
3483 bulk_00002.hld	2511.683100	503833.379805	360.059044	136788292.963455	3523.070613	3561.163847	27.276214	3.683308	116.565158	1971.915616	1.135739	-134.199000	-88.703500	-0.179136
3483 bulk_00003.hld	2450.729390	535856.608520	357.418797	130089907.268479	3525.486809	3575.159498	27.764536	4.119125	92.387596	1834.142611	1.161266	-134.099000	-88.703500	-0.262651
3483 bulk_00004.hld	2508.900103	518971.542614	366.247506	136478639.992633	3522.291127	3571.647700	27.776477	3.802584	132.867618	1981.856593	1.121944	-133.999000	-88.703500	-0.245266
3483 bulk_00005.hld	2480.324020	490765.470487	334.223870	133320248.777579	3521.421989	3581.604136	25.646271	3.681102	122.006597	1936.016372	1.120687	-134.399000	-88.603500	-0.149573
3483 bulk_00006.hld	2472.360932	489614.479231	331.352726	132446990.227038	3522.221399	3580.578340	25.509640	3.696683	129.377213	1936.581618	1.112595	-134.299000	-88.603500	-0.195713
3483 bulk_00007.hld	2462.380764	485279.745613	326.605224	131356757.213953	3521.082742	3576.753048	25.248277	3.694365	162.004833	1966.081807	1.084021	-134.199000	-88.603500	-0.139017
3483 bulk_00008.hld	2454.265181	499714.159769	332.703611	130473675.800001	3522.269859	3580.750160	25.806606	3.830000	127.252820	1906.304340	1.114826	-134.099000	-88.603500	-0.088466
3483 bulk_00009.hld	2476.891305	506701.878966	343.873233	132943438.903712	3523.159269	3582.026492	26.424072	3.811409	129.269792	1935.898509	1.117145	-133.999000	-88.603500	-0.092392
3483 bulk_00010.hld	2469.410620	492255.835000	327.010720	132124208.959261	3523.413426	3598.400753	25.206098	3.725705	101.541287	1883.082618	1.139504	-134.399000	-88.503500	-0.104227
3483 bulk_00011.hld	2449.728715	485755.003095	318.289203	129981402.887213	3521.914617	3594.336352	24.735240	3.737112	153.035260	1934.718349	1.087459	-134.299000	-88.503500	-0.130152
3483 bulk_00012.hld	2436.956091	490200.927490	317.434342	128600600.300286	3522.587718	3595.150551	24.800888	3.811809	148.042475	1910.436557	1.090953	-134.199000	-88.503500	-0.046195
3483 bulk_00013.hld	2427.740221	497186.952423	319.574466	127609083.873376	3521.072831	3594.573787	25.064907	3.896172	126.224830	1866.810741	1.110546	-134.099000	-88.503500	-0.044524
3483 bulk_00014.hld	2438.597217	496772.246827	323.116026	128777585.704355	3521.842350	3591.678941	25.227440	3.857599	145.793594	1908.299028	1.094922	-133.999000	-88.503500	-0.019217
3483 bulk_00015.hld	2447.071196	479250.924940	310.280223	129693474.101359	3522.226622	3605.502082	24.139588	3.695259	121.752624	1888.835821	1.111417	-134.399000	-88.403500	-0.047708
3483 bulk_00016.hld	2440.129959	489715.251399	314.073430	128942997.350889	3524.091519	3609.558517	24.505702	3.797920	111.482201	1858.313275	1.123142	-134.299000	-88.403500	-0.005432
3483 bulk_00017.hld	2424.384384	472658.705910	301.291355	127249030.874448	3521.550455	3600.966529	23.664332	3.714439	198.826582	1954.402328	1.049585	-134.199000	-88.403500	-0.018422
3483 bulk_00018.hld	2421.920606	482880.654782	306.903643	126985026.312185	3521.335703	3601.966850	24.130183	3.802658	162.574919	1909.526988	1.075661	-134.099000	-88.403500	-0.018786
3483 bulk_00019.hld	2431.581708	491523.600069	314.761468	128021894.721387	3521.502985	3602.762865	24.647579	3.839371	161.388498	1916.890561	1.079597	-133.999000	-88.403500	-0.045856
3483 bulk_00020.hld	2406.432253	491067.280215	302.694027	125331935.365115	3524.139551	3623.174004	23.955642	3.918134	72.432870	1726.993932	1.168806	-134.399000	-88.303500	-0.044165
3483 bulk_00021.hld	2392.842330	461784.301601	284.013287	123890778.526887	3521.370776	3612.286075	22.607576	3.727350	223.756205	1940.246672	1.028362	-134.299000	-88.303500	-0.047619
3483 bulk_00022.hld	2394.643140	469510.816622	289.229951	124081246.962877	3521.359224	3612.128089	23.005147	3.783898	204.670643	1922.083887	1.041108	-134.199000	-88.303500	-0.019270
3483 bulk_00023.hld	2402.863781	479276.533394	296.701412	124952670.668174	3522.156978	3614.376048	23.516987	3.835665	190.546675	1914.002107	1.052635	-134.099000	-88.303500	-0.036806
3483 bulk_00024.hld	2419.278445	485551.766509	304.949880	126702225.279422	3522.044571	3613.454436	24.003312	3.832228	156.866576	1895.385793	1.079030	-133.999000	-88.303500	-0.047977