Fri Aug 26 10:55:52 2022

Number of Points = 9926

Depth (nm)	Load (N)	Time (s)
1.730028	99.392289	0.000000
1.274504	96.945182	0.005005
1.246444	97.446493	0.010010
1.524424	90.541472	0.015014
1.105528	93.375146	0.020019
0.840842	77.038321	0.025024
0.710935	89.833664	0.030029
0.001213	80.380659	0.035034
0.010565	59.271511	0.040038
-0.746000	66.479312	0.045043
-0.268597	63.048587	0.050048
-0.778295	51.375203	0.055053
-1.118842	49.008275	0.060058
-1.178224	39.628038	0.065062
-1.710682	35.285235	0.070067
-1.493814	27.861423	0.075072
-1.739643	31.107889	0.080077
-2.162107	29.291539	0.085082
-2.051327	15.607563	0.090086
-2.822371	20.460681	0.095091
-3.331409	8.337985	0.100096
-3.612266	11.482337	0.105101
-4.152521	19.741572	0.110106
-4.216697	2.573194	0.115110
-4.558511	8.545847	0.120115
-4.404377	6.639725	0.125120
-4.750857	-1.012729	0.130125
-5.029753	4.649580	0.135130
-5.298770	-10.731066	0.140134
-5.962782	-5.562437	0.145139
-6.327961	-2.847870	0.150144
-6.338424	-8.357066	0.155149
-6.530226	-8.013755	0.160154
-6.260149	-10.292255	0.165158
-6.838500	-9.505959	0.170163
-7.749142	-11.648080	0.175168
-7.742704	-8.475698	0.180173
-7.857379	0.900470	0.185178
-7.530570	-3.484362	0.190182
-7.758520	1.353792	0.195187
-8.023578	-5.631152	0.200192
-8.583499	2.077499	0.205197
-9.386348	-10.511948	0.210202
-9.215342	-5.403729	0.215206
-9.325770	-10.742341	0.220211
-9.395519	-2.600664	0.225216
-10.074955	-9.897563	0.230221
-10.438499	-1.425414	0.235226
-10.599643	-11.966655	0.240230
-10.922708	-6.778347	0.245235
-10.844343	-4.775058	0.250240
-11.078526	-5.057878	0.255245
-11.825562	4.204785	0.260250
-11.495553	-11.958802	0.265254
-11.986107	-6.073723	0.270259
-12.167090	-3.112598	0.275264
-12.011016	0.099760	0.280269
-12.480769	-5.148107	0.285274
-12.996345	-9.291054	0.290278
-13.208418	1.783339	0.295283
-13.289674	-3.319380	0.300288
-13.376949	-2.391251	0.305293
-14.394399	1.880152	0.310298
-14.399362	-5.616671	0.315302
-14.760747	1.558048	0.320307
-14.902028	-4.288273	0.325312
-14.929895	0.550365	0.330317
-15.600875	0.626609	0.335322
-14.975215	-1.156781	0.340326
-15.792532	-4.708601	0.345331
-16.298548	-8.002015	0.350336
-16.400422	-6.195283	0.355341
-16.590248	-3.561800	0.360346
-16.580623	-5.904149	0.365350
-16.756456	3.285396	0.370355
-17.036941	1.004033	0.375360
-17.366868	2.131289	0.380365
-17.759921	1.205675	0.385370
-17.653084	-6.539501	0.390374
-17.845628	-0.397110	0.395379
-18.409243	-2.409771	0.400384
-18.863875	-5.685877	0.405389
-19.343388	-3.823511	0.410394
-19.143889	-12.165222	0.415398
-19.000133	-2.778675	0.420403
-19.506246	-1.355077	0.425408
-20.217719	-6.296399	0.430413
-20.567763	0.316588	0.435418
-20.443793	-6.510634	0.440422
-20.674582	-0.684981	0.445427
-20.814154	-0.286528	0.450432
-21.104447	-5.467427	0.455437
-21.933549	1.514367	0.460442
-21.474250	-0.568977	0.465446
-21.963463	-1.394200	0.470451
-22.076978	-4.619016	0.475456
-21.926503	-10.178578	0.480461
-23.332473	-5.656867	0.485466
-23.474802	-6.605698	0.490470
-23.666236	-4.174438	0.495475
-23.650250	-6.796179	0.500480
-23.691562	-0.810208	0.505485
-23.888059	-2.842064	0.510490
-23.689449	-9.200032	0.515494
-24.050067	1.840542	0.520499
-25.061428	-0.589607	0.525504
-24.713612	-4.139344	0.530509
-25.055399	0.137587	0.535514
-25.369055	-6.150114	0.540518
-26.436822	0.622075	0.545523
-26.231220	0.441619	0.550528
-26.281877	-5.346047	0.555533
-26.429571	5.512687	0.560538
-26.302852	-9.825173	0.565542
-26.477918	-4.938308	0.570547
-27.217456	8.755457	0.575552
-27.345123	-1.129799	0.580557
-28.039846	-3.685175	0.585562
-27.737911	-0.656874	0.590566
-28.315579	2.540016	0.595571
-28.899257	1.454263	0.600576
-29.064075	1.296681	0.605581
-29.373077	4.809233	0.610586
-29.071748	7.543410	0.615590
-29.391422	4.081781	0.620595
-29.482947	0.008846	0.625600
-29.521321	-0.092496	0.630605
-30.524596	12.041529	0.635610
-30.529459	-3.592212	0.640614
-31.371113	5.188489	0.645619
-30.985057	-3.849802	0.650624
-31.028877	-4.428006	0.655629
-31.532623	6.055908	0.660634
-31.751898	-2.752098	0.665638
-32.321398	4.727098	0.670643
-32.371546	-1.000539	0.675648
-32.087454	-2.417547	0.680653
-32.375466	9.326711	0.685658
-32.725312	-12.302205	0.690662
-33.607305	3.375196	0.695667
-33.843659	1.055326	0.700672
-33.864192	-0.829927	0.705677
-34.210892	-1.497011	0.710682
-33.645260	-3.055927	0.715686
-34.286793	0.470434	0.720691
-34.843865	0.057560	0.725696
-34.834964	-3.414099	0.730701
-35.158188	-1.901921	0.735706
-35.279386	-15.489642	0.740710
-36.292934	-1.841804	0.745715
-36.403233	1.389881	0.750720
-36.474860	-10.079591	0.755725
-36.704984	8.615673	0.760730
-36.552791	-6.836881	0.765734
-37.029822	1.947157	0.770739
-37.288605	0.086344	0.775744
-37.516735	-4.942887	0.780749
-38.137360	2.060231	0.785754
-38.132265	-0.664215	0.790758
-38.206019	-2.727837	0.795763
-38.090386	-4.058506	0.800768
-38.380915	-12.149920	0.805773
-39.488384	0.800723	0.810778
-39.924294	-8.068460	0.815782
-39.776643	-2.428276	0.820787
-40.114398	-0.157725	0.825792
-39.507788	-7.762421	0.830797
-39.795815	2.317757	0.835802
-40.127215	-5.545841	0.840806
-40.873808	-5.954515	0.845811
-41.277654	2.789655	0.850816
-41.140592	-4.074405	0.855821
-41.765381	-2.879094	0.860826
-41.286518	-4.712393	0.865830
-42.017203	-3.462630	0.870835
-42.410604	-7.665725	0.875840
-42.574787	-6.924931	0.880845
-42.776652	0.101567	0.885850
-42.759286	-9.575318	0.890854
-43.548768	3.518798	0.895859
-44.442851	1.643009	0.900864
-43.807813	-12.002348	0.905869
-44.283547	6.237625	0.910874
-44.350570	-1.347608	0.915878
-44.448005	-6.242169	0.920883
-44.394890	-7.613723	0.925888
-44.412841	-10.369379	0.930893
-45.446084	4.363495	0.935898
-45.756393	-6.619577	0.940902
-46.001381	-6.657113	0.945907
-45.898432	5.570416	0.950912
-45.561614	-3.513990	0.955917
-46.439692	6.379659	0.960922
-47.196718	0.499499	0.965926
-47.741196	2.432090	0.970931
-47.568464	0.374382	0.975936
-47.406599	-2.260581	0.980941
-47.670345	-0.817774	0.985946
-47.974030	-4.019308	0.990950
-48.434026	-3.077437	0.995955
-48.738651	2.898913	1.000960
-48.543802	-6.068478	1.005965
-48.620948	-2.841955	1.010970
-49.374325	-5.277471	1.015974
-49.737396	-10.260380	1.020979
-50.294655	0.516589	1.025984
-50.024271	-5.928481	1.030989
-50.500398	7.335140	1.035994
-50.321923	-3.211526	1.040998
-50.463060	-0.712169	1.046003
-50.602031	-1.471705	1.051008
-51.083649	-9.830749	1.056013
-51.701003	-3.919601	1.061018
-52.003965	0.028592	1.066022
-51.969718	-8.015316	1.071027
-52.044325	2.363814	1.076032
-53.022643	-1.931702	1.081037
-53.253194	8.215456	1.086042
-52.996254	3.980702	1.091046
-53.612466	-4.607316	1.096051
-53.457060	5.666403	1.101056
-53.412500	-1.123146	1.106061
-54.221862	-1.382847	1.111066
-54.253361	-1.925006	1.116070
-54.408802	3.876261	1.121075
-54.674454	3.142776	1.126080
-54.650637	-12.571347	1.131085
-55.482281	6.217567	1.136090
-55.916518	0.296642	1.141094
-56.173864	0.545758	1.146099
-56.187988	2.794393	1.151104
-56.202177	0.025495	1.156109
-56.369730	1.092670	1.161114
-56.509871	-3.754114	1.166118
-57.493243	-0.041656	1.171123
-57.896716	-9.564433	1.176128
-57.757246	-7.539024	1.181133
-58.219168	2.020917	1.186138
-58.132883	-0.700351	1.191142
-58.059405	2.458429	1.196147
-58.221111	0.845085	1.201152
-58.566099	-2.302563	1.206157
-59.576695	4.397453	1.211162
-59.533563	3.894292	1.216166
-59.630501	5.956512	1.221171
-59.644490	-0.643593	1.226176
-59.282882	-9.377527	1.231181
-60.157920	-2.005781	1.236186
-60.477784	1.236387	1.241190
-60.606854	3.211864	1.246195
-60.803023	0.385882	1.251200
-61.486465	3.611896	1.256205
-62.190114	3.281953	1.261210
-62.251333	-9.460922	1.266214
-62.090181	-0.826870	1.271219
-62.744317	-2.578671	1.276224
-62.381596	-0.464638	1.281229
-62.689898	0.254305	1.286234
-62.695891	7.262962	1.291238
-63.579412	0.314204	1.296243
-64.330789	3.648868	1.301248
-63.955583	-5.912895	1.306253
-64.326532	0.197162	1.311258
-64.174518	-0.139461	1.316262
-64.461618	6.444745	1.321267
-64.489119	1.985369	1.326272
-65.201407	5.013401	1.331277
-65.327588	4.435365	1.336282
-65.716594	7.409899	1.341286
-65.841124	14.041559	1.346291
-66.111523	8.892361	1.351296
-65.800765	-2.196903	1.356301
-66.786767	-0.208221	1.361306
-66.905474	1.427131	1.366310
-67.078528	-1.285395	1.371315
-67.409279	8.526200	1.376320
-67.645449	2.919272	1.381325
-68.053741	0.502792	1.386330
-68.055907	1.145596	1.391334
-68.310466	1.001987	1.396339
-68.537017	2.113147	1.401344
-68.613287	-1.329432	1.406349
-68.982996	10.898927	1.411354
-69.760931	-3.393274	1.416358
-69.582988	-4.543827	1.421363
-69.879453	0.621358	1.426368
-70.008849	-10.465805	1.431373
-70.314723	1.509008	1.436378
-70.659688	-1.211551	1.441382
-71.143908	2.600354	1.446387
-71.688132	-2.490388	1.451392
-71.794162	-1.534029	1.456397
-71.800764	5.405122	1.461402
-71.648725	2.436342	1.466406
-71.423245	4.445197	1.471411
-71.569618	-0.141198	1.476416
-71.893272	-3.652822	1.481421
-72.415226	-8.019392	1.486426
-72.819930	-4.934852	1.491430
-73.628462	-1.328707	1.496435
-73.931122	-3.277596	1.501440
-73.820568	-3.288235	1.506445
-73.770168	-1.388157	1.511450
-74.172634	-5.134274	1.516454
-75.058556	-6.103365	1.521459
-75.024796	-6.744267	1.526464
-75.387707	-0.796808	1.531469
-75.781097	11.846512	1.536474
-75.731469	-1.226828	1.541478
-75.692627	-3.238379	1.546483
-75.785473	3.097288	1.551488
-76.265496	-3.604254	1.556493
-76.923846	0.807383	1.561498
-76.778704	-2.533633	1.566502
-77.120823	-7.061075	1.571507
-77.168771	-6.869871	1.576512
-77.878502	-8.647815	1.581517
-78.208079	-1.791253	1.586522
-78.422034	-4.614465	1.591526
-78.536725	-1.344133	1.596531
-78.920386	4.935578	1.601536
-78.677214	-10.439388	1.606541
-78.821356	-4.889812	1.611546
-79.122707	3.642253	1.616550
-79.569604	-9.239881	1.621555
-80.209840	7.655844	1.626560
-79.977163	-10.109205	1.631565
-80.763096	2.408572	1.636570
-80.773656	-13.189467	1.641574
-80.401449	-9.738692	1.646579
-81.325954	-2.333936	1.651584
-81.529524	-7.259424	1.656589
-81.485360	-6.405542	1.661594
-81.495267	-2.291014	1.666598
-81.741848	-1.410845	1.671603
-82.592171	-1.227584	1.676608
-83.049116	-6.436314	1.681613
-83.227222	-3.304800	1.686618
-82.927289	-8.669339	1.691622
-83.159319	-9.863622	1.696627
-83.427059	6.100938	1.701632
-83.788899	-14.298603	1.706637
-84.642639	-1.684853	1.711642
-84.799281	6.565262	1.716646
-84.774705	3.483455	1.721651
-85.034619	4.656756	1.726656
-84.922455	-3.946594	1.731661
-84.799447	2.222591	1.736666
-85.351585	-6.264672	1.741670
-85.755538	0.521216	1.746675
-86.117226	4.064115	1.751680
-86.257679	0.100038	1.756685
-86.864457	3.314115	1.761690
-87.231029	-1.601814	1.766694
-87.655730	-7.147746	1.771699
-87.472860	-3.385925	1.776704
-87.585790	-8.559635	1.781709
-87.940187	-4.793254	1.786714
-87.700685	-11.777659	1.791718
-88.507258	-8.317348	1.796723
-88.908675	-2.730877	1.801728
-89.018865	-2.659692	1.806733
-89.379773	0.835631	1.811738
-89.260817	7.597050	1.816742
-89.675549	2.283673	1.821747
-89.760091	-1.540419	1.826752
-90.167578	-2.897202	1.831757
-90.520997	4.712857	1.836762
-90.519630	3.437942	1.841766
-90.627674	2.436318	1.846771
-91.037809	-3.273229	1.851776
-91.597988	-1.860194	1.856781
-91.894055	-0.425009	1.861786
-92.164357	-1.834789	1.866790
-92.406823	0.493689	1.871795
-92.531771	-1.656870	1.876800
-92.463784	-1.053461	1.881805
-92.707636	1.901634	1.886810
-93.199363	-4.469064	1.891814
-93.742106	-10.464835	1.896819
-93.802270	-4.276624	1.901824
-94.181927	2.850318	1.906829
-94.071114	3.156004	1.911834
-94.077458	-1.354119	1.916838
-94.059157	-5.184731	1.921843
-95.089459	-6.099705	1.926848
-94.913602	-11.489214	1.931853
-95.500034	-5.804338	1.936858
-95.581688	-4.677774	1.941862
-95.730484	-8.453896	1.946867
-96.149473	-5.655024	1.951872
-96.465200	-3.704268	1.956877
-96.484505	-1.382063	1.961882
-96.503858	-0.249382	1.966886
-97.400716	-5.092233	1.971891
-97.887464	0.694179	1.976896
-97.780704	3.313120	1.981901
-97.976143	2.533904	1.986906
-98.257554	7.275981	1.991910
-97.803912	-0.583299	1.996915
-98.952283	0.995814	2.006912
-98.583343	-2.792681	2.016909
-98.338195	0.495723	2.026906
-97.329884	-1.751457	2.036902
-96.879088	2.331696	2.046899
-96.330525	1.787462	2.056896
-95.890070	-6.298060	2.066893
-95.825189	1.060391	2.076890
-94.855266	7.970663	2.086886
-94.318325	3.623834	2.096883
-94.425038	6.929012	2.106880
-93.422601	-0.924076	2.116877
-93.184851	3.214423	2.126874
-92.342535	5.738298	2.136870
-91.632144	-0.181372	2.146867
-91.426360	2.397263	2.156864
-90.868301	-1.860989	2.166861
-90.146634	1.676327	2.176858
-89.981455	-0.648645	2.186854
-89.754538	1.758811	2.196851
-88.786114	-2.446130	2.206848
-88.715311	8.747482	2.216845
-87.709820	6.440554	2.226842
-87.009898	-0.839595	2.236838
-87.161006	-0.666692	2.246835
-86.637457	2.055696	2.256832
-86.027209	-0.249878	2.266829
-85.561659	-1.139136	2.276826
-84.827239	-2.238145	2.286822
-84.485295	-2.880084	2.296819
-83.854533	-0.887120	2.306816
-82.989105	4.886380	2.316813
-82.715004	5.930716	2.326810
-82.585052	9.430288	2.336806
-82.342031	4.128231	2.346803
-81.580948	2.987058	2.356800
-80.633544	6.112271	2.366797
-80.065534	3.274765	2.376794
-80.129835	0.342480	2.386790
-79.691279	-3.013377	2.396787
-78.595154	-4.593175	2.406784
-78.414818	1.445378	2.416781
-78.258657	-5.373150	2.426778
-77.380379	-3.773507	2.436774
-76.745696	-6.355306	2.446771
-76.388950	-3.499246	2.456768
-75.610368	-6.087612	2.466765
-75.534873	-6.415642	2.476762
-74.908283	-3.965881	2.486758
-74.190029	-2.075236	2.496755
-73.793558	-6.282986	2.506752
-74.030316	-5.140104	2.516749
-73.234688	-4.218150	2.526746
-72.181402	-5.740593	2.536742
-71.445043	-5.246553	2.546739
-71.517190	0.847150	2.556736
-71.385220	3.978955	2.566733
-70.314529	-4.841404	2.576730
-70.058093	-1.507241	2.586726
-68.872529	0.054061	2.596723
-68.760858	-7.758531	2.606720
-68.772037	0.321327	2.616717
-67.927276	-0.760017	2.626714
-67.543142	-4.538208	2.636710
-66.930700	2.845860	2.646707
-65.785278	-3.971479	2.656704
-65.767609	3.327804	2.666701
-65.536884	4.831874	2.676698
-65.085534	1.081229	2.686694
-64.424813	1.916487	2.696691
-63.701110	0.286974	2.706688
-63.044347	-3.625528	2.716685
-62.573352	1.886281	2.726682
-62.447246	1.506022	2.736678
-62.316724	1.102903	2.746675
-61.367313	4.050414	2.756672
-61.189986	5.401246	2.766669
-60.237528	-2.887538	2.776666
-59.590885	-0.497916	2.786662
-59.673423	-1.336682	2.796659
-58.763638	1.420601	2.806656
-58.378514	3.860445	2.816653
-57.860014	-3.784251	2.826650
-56.858933	0.039002	2.836646
-56.605952	-4.931997	2.846643
-56.741104	-2.566365	2.856640
-56.232196	-3.690447	2.866637
-55.333123	-0.098392	2.876634
-54.639756	-4.564605	2.886630
-53.927241	-3.933808	2.896627
-53.989030	-1.598605	2.906624
-53.824043	-1.975414	2.916621
-52.704986	-0.156675	2.926618
-52.424633	1.783147	2.936614
-51.673122	-6.401492	2.946611
-50.962481	-8.016300	2.956608
-50.814140	-6.024248	2.966605
-50.692956	-4.278216	2.976602
-49.804692	-3.715963	2.986598
-49.369379	-7.540134	2.996595
-49.021032	-3.250966	3.006592
-48.361256	-4.284502	3.016589
-48.038139	-5.164253	3.026586
-47.119617	-1.515039	3.036582
-46.659511	2.009153	3.046579
-46.515561	-9.121878	3.056576
-45.661499	-5.202877	3.066573
-45.300215	-6.367329	3.076570
-44.845671	-11.043436	3.086566
-44.354030	0.087819	3.096563
-43.857270	0.125005	3.106560
-43.281704	-7.300501	3.116557
-42.227786	-0.742249	3.126554
-42.350306	-8.626082	3.136550
-42.357542	-6.071299	3.146547
-41.423470	-6.833939	3.156544
-40.927113	-3.613156	3.166541
-40.019612	-13.941267	3.176538
-39.187184	-6.651639	3.186534
-39.180745	-10.396364	3.196531
-39.198077	-7.624606	3.206528
-38.480585	-8.030420	3.216525
-37.970097	-9.427170	3.226522
-37.264493	-3.875864	3.236518
-36.256533	-2.001814	3.246515
-36.123054	2.669257	3.256512
-36.171374	-1.323528	3.266509
-35.329657	-0.548127	3.276506
-34.650195	-6.063850	3.286502
-34.627466	-3.291993	3.296499
-33.771840	1.253970	3.306496
-33.380721	0.179904	3.316493
-32.813728	-2.929865	3.326490
-31.799196	-6.847388	3.336486
-31.370972	-8.658968	3.346483
-31.401952	-5.875581	3.356480
-31.308611	-1.477019	3.366477
-30.477737	0.617833	3.376474
-29.574711	-1.955064	3.386470
-28.864455	-5.432418	3.396467
-28.557585	-2.109273	3.406464
-28.920576	2.632762	3.416461
-27.594399	-5.004645	3.426458
-27.097713	-3.659189	3.436454
-27.127205	-0.201313	3.446451
-25.932260	0.303689	3.456448
-25.999297	-4.069473	3.466445
-25.505454	-2.615872	3.476442
-24.730624	-2.023286	3.486438
-24.422486	-2.726482	3.496435
-23.508698	-1.632861	3.506432
-23.018082	4.781858	3.516429
-22.862649	6.595417	3.526426
-22.372809	-0.256063	3.536422
-21.460803	1.626592	3.546419
-21.522081	-5.459015	3.556416
-20.890169	3.876495	3.566413
-20.374602	-0.067876	3.576410
-19.819873	5.313695	3.586406
-18.976287	1.416451	3.596403
-18.650516	-2.954516	3.606400
-18.570668	0.514845	3.616397
-17.468360	3.150293	3.626394
-17.014387	-2.190945	3.636390
-17.035897	-1.810146	3.646387
-16.288204	1.133930	3.656384
-15.598692	-3.296839	3.666381
-15.431627	-3.252668	3.676378
-14.767559	-6.846370	3.686374
-13.977949	-6.940307	3.696371
-13.875861	-5.840679	3.706368
-13.123478	-6.666893	3.716365
-12.723411	-3.643352	3.726362
-12.623873	-9.043441	3.736358
-11.983970	-0.377560	3.746355
-11.035340	-5.691280	3.756352
-10.435040	-4.175061	3.766349
-10.302010	-6.304966	3.776346
-9.985502	2.506299	3.786342
-9.028999	1.660974	3.796339
-8.592316	1.292547	3.806336
-8.249528	5.243640	3.816333
-7.969827	6.467665	3.826330
-7.076137	12.677085	3.836326
-6.922325	8.516614	3.846323
-5.988166	19.734204	3.856320
-5.618603	21.276848	3.866317
-5.675323	16.449092	3.876314
-4.989217	31.367174	3.886310
-4.547036	27.969565	3.896307
-4.390652	43.591004	3.906304
-3.630754	51.439966	3.916301
-2.863945	55.572134	3.926298
-2.225740	70.060563	3.936294
-2.186230	73.007212	3.946291
-1.233604	90.950193	3.956288
-1.101397	93.914090	3.966285
-0.651310	105.660087	3.976282
0.000000	106.789837	3.981286
-0.071198	118.895871	3.986291
0.448540	120.055355	3.991296
0.517605	125.859673	3.996301
0.197333	127.146781	4.001306
0.437409	118.368430	4.006310
0.495695	123.200016	4.011315
0.841865	118.739375	4.016320
0.562160	113.132860	4.021325
0.309617	117.145994	4.026330
0.704015	120.941347	4.031334
0.457667	120.932494	4.036339
0.649408	114.411040	4.041344
0.597541	121.113686	4.046349
0.295216	127.061248	4.051354
0.540653	123.653973	4.056358
0.874227	133.011039	4.061363
0.644069	136.457559	4.066368
0.690268	135.852679	4.071373
0.897186	136.529372	4.076378
0.580919	130.447666	4.081382
0.809601	140.165908	4.086387
0.778064	130.455430	4.091392
1.028754	134.567382	4.096397
0.383216	125.069560	4.101402
1.024770	133.435902	4.106406
0.981289	133.022151	4.111411
0.583046	125.241664	4.116416
0.965657	135.445287	4.121421
1.201572	136.705909	4.126426
0.424840	123.523855	4.131430
0.641513	139.666217	4.136435
0.847878	135.869564	4.141440
0.890012	129.662455	4.146445
1.010526	139.856271	4.151450
1.137450	138.302375	4.156454
1.217313	137.746036	4.161459
1.155108	129.720243	4.166464
0.792692	119.808194	4.171469
0.869574	125.212673	4.176474
0.923041	117.583316	4.181478
1.373489	138.453764	4.186483
0.875156	130.654058	4.191488
0.963271	128.185577	4.196493
0.747364	129.734839	4.201498
0.992902	134.065886	4.206502
1.582511	140.111857	4.211507
1.034573	125.951404	4.216512
0.856842	129.253722	4.221517
1.094067	134.974916	4.226522
1.385118	132.180617	4.231526
1.123413	136.062308	4.236531
0.811627	131.103007	4.241536
1.166791	129.254155	4.246541
1.113095	139.829425	4.251546
1.514412	141.804594	4.256550
1.162190	136.177725	4.261555
1.450030	136.800692	4.266560
1.164027	125.120904	4.271565
1.064018	127.901770	4.276570
1.117840	125.568340	4.281574
1.337279	134.462300	4.286579
1.497899	135.899155	4.291584
1.355271	129.290554	4.296589
1.068367	123.273879	4.301594
1.166370	125.277289	4.306598
1.316324	138.601717	4.311603
1.361678	134.323946	4.316608
2.002809	134.316118	4.321613
1.368872	126.284433	4.326618
1.511508	118.628538	4.331622
1.290813	125.677001	4.336627
0.892077	127.463530	4.341632
0.978173	131.822565	4.346637
1.484251	141.209724	4.351642
1.573033	136.333584	4.356646
1.722461	143.631304	4.361651
1.583926	130.767484	4.366656
1.342425	123.851585	4.371661
1.192486	125.428539	4.376666
1.928906	124.096115	4.381670
1.350207	132.617646	4.386675
1.294778	121.768807	4.391680
1.039779	128.974468	4.396685
1.692709	132.618843	4.401690
1.931767	125.020697	4.406694
2.019275	136.640137	4.411699
1.617009	133.254614	4.416704
1.304277	120.101557	4.421709
1.276239	131.501709	4.426714
1.951933	141.330682	4.431718
1.749042	132.725694	4.436723
1.682645	127.718697	4.441728
1.270881	130.883452	4.446733
1.524245	135.871325	4.451738
1.779670	132.231545	4.456742
1.682737	141.734737	4.461747
1.758420	147.392503	4.466752
2.049640	152.415614	4.471757
1.526518	148.700900	4.476762
1.814097	145.125712	4.481766
1.583010	148.923547	4.486771
1.959804	139.222253	4.491776
1.972596	137.626017	4.496781
1.705913	147.386589	4.501786
1.853480	139.309149	4.506790
1.850664	137.816582	4.511795
1.937971	133.959374	4.516800
1.702228	133.338282	4.521805
1.492220	149.480648	4.526810
1.905441	144.386317	4.531814
1.939256	141.084752	4.536819
1.746609	154.048092	4.541824
1.882545	147.560624	4.546829
1.899726	142.765231	4.551834
1.874505	141.665283	4.556838
1.694188	152.927811	4.561843
1.864534	148.001004	4.566848
1.950365	153.964069	4.571853
1.852808	146.045010	4.576858
1.912321	142.631879	4.581862
1.654927	142.396962	4.586867
1.716505	142.147182	4.591872
1.999604	146.459730	4.596877
1.744058	144.459195	4.601882
2.016878	140.791396	4.606886
2.022862	149.592051	4.611891
1.767077	145.066942	4.616896
2.344867	150.937591	4.621901
2.183331	151.029425	4.626906
2.431905	137.703543	4.631910
1.689839	143.156442	4.636915
1.820531	146.084885	4.641920
2.395928	152.019180	4.646925
2.264227	159.819410	4.651930
2.303419	155.419210	4.656934
2.117403	152.974425	4.661939
2.389210	152.619149	4.666944
2.039766	141.221305	4.671949
1.775718	162.661758	4.676954
2.380145	155.168060	4.681958
2.593498	159.500962	4.686963
2.527934	159.049520	4.691968
2.494185	146.466760	4.696973
2.315158	148.497486	4.701978
2.131517	140.228011	4.706982
1.847246	142.892039	4.711987
2.225851	159.395174	4.716992
2.659887	157.948481	4.721997
2.405368	163.334969	4.727002
2.184679	149.553806	4.732006
2.365085	153.262264	4.737011
2.461714	162.305070	4.742016
2.516788	159.613945	4.747021
2.018086	167.569393	4.752026
2.612422	155.154585	4.757030
2.599308	163.743090	4.762035
2.526103	161.837547	4.767040
2.198034	159.829320	4.772045
2.273370	156.739581	4.777050
2.849779	155.504833	4.782054
2.651809	167.095977	4.787059
2.608343	161.930380	4.792064
2.351367	155.279463	4.797069
2.377736	164.080115	4.802074
2.738109	159.756453	4.807078
2.774631	167.135036	4.812083
2.533934	157.536200	4.817088
2.494194	161.870543	4.822093
2.460283	160.341687	4.827098
2.561740	157.368101	4.832102
2.529272	159.388665	4.837107
2.791967	161.167125	4.842112
2.884573	163.449783	4.847117
2.465507	166.625171	4.852122
2.981629	167.089213	4.857126
2.784333	165.959109	4.862131
2.647924	156.780623	4.867136
2.836416	157.191274	4.872141
2.445513	158.112903	4.877146
2.609440	152.722034	4.882150
2.601369	157.446905	4.887155
2.570015	160.887786	4.892160
2.931625	156.022944	4.897165
2.465752	164.621833	4.902170
2.802379	158.653594	4.907174
2.666692	161.335619	4.912179
2.646230	157.583769	4.917184
2.881160	160.388419	4.922189
2.355832	167.734259	4.927194
2.721035	156.541505	4.932198
2.840178	157.677943	4.937203
2.639023	158.044859	4.942208
2.795095	163.642659	4.947213
2.735472	162.896071	4.952218
2.917020	161.744946	4.957222
2.699186	176.158024	4.962227
3.042254	183.485721	4.967232
3.298504	185.065876	4.972237
3.063805	181.496069	4.977242
3.168309	172.213629	4.982246
2.966383	165.323189	4.987251
2.819729	168.266344	4.992256
2.930185	160.384493	4.997261
3.005678	172.002663	5.002266
3.089097	173.562270	5.007270
2.788840	170.860030	5.012275
3.009669	177.406346	5.017280
3.526798	179.720984	5.022285
2.834503	193.556230	5.027290
2.937226	186.763878	5.032294
3.237537	190.558076	5.037299
3.352267	191.078286	5.042304
3.441118	178.985767	5.047309
2.968451	182.501691	5.052314
3.157393	192.311568	5.057318
3.510481	189.687931	5.062323
3.286774	182.370615	5.067328
3.177731	170.172875	5.072333
3.015716	178.730788	5.077338
3.218280	176.532377	5.082342
3.322786	184.843158	5.087347
3.209653	186.189765	5.092352
3.306877	186.317241	5.097357
3.375796	186.407995	5.102362
3.720643	183.744514	5.107366
3.440679	168.776694	5.112371
3.160707	167.346258	5.117376
2.788442	165.322766	5.122381
3.361539	188.951886	5.127386
3.292548	186.558478	5.132390
3.457070	185.128435	5.137395
3.412796	178.789234	5.142400
3.795678	185.886112	5.147405
3.143418	185.522852	5.152410
3.446106	186.494677	5.157414
3.712641	191.967722	5.162419
3.333913	176.904543	5.167424
3.078105	176.713670	5.172429
2.931820	196.297732	5.177434
3.282687	187.385041	5.182438
3.221118	190.960343	5.187443
2.941876	190.431441	5.192448
3.289256	181.626862	5.197453
2.928803	189.453230	5.202458
3.508038	195.870985	5.207462
4.023960	199.745509	5.212467
3.865982	195.293742	5.217472
3.936930	188.322843	5.222477
3.137628	187.859093	5.227482
3.477431	176.613335	5.232486
3.794742	192.759058	5.237491
3.355436	203.150800	5.242496
4.143955	200.845336	5.247501
3.716543	193.455330	5.252506
3.609497	194.857936	5.257510
3.657859	180.917803	5.262515
3.462099	188.731183	5.267520
4.052430	186.478723	5.272525
3.682830	185.131842	5.277530
4.330312	190.029894	5.282534
3.852569	188.029149	5.287539
3.654205	182.381474	5.292544
3.925034	179.267621	5.297549
3.497615	189.059570	5.302554
3.744505	190.691801	5.307558
3.878527	185.030338	5.312563
3.826865	193.039578	5.317568
3.914552	177.479847	5.322573
3.456207	186.896967	5.327578
3.657916	194.778176	5.332582
4.008080	205.942325	5.337587
4.127992	208.116336	5.342592
4.029690	201.472333	5.347597
3.822026	204.554704	5.352602
3.782232	195.908473	5.357606
3.564968	198.663315	5.362611
3.745653	207.180540	5.367616
3.975187	205.759355	5.372621
3.915669	215.316871	5.377626
3.971897	217.829821	5.382630
3.767297	221.652020	5.387635
3.427547	220.471327	5.392640
4.007743	205.872578	5.397645
3.826439	210.953458	5.402650
4.087211	216.364134	5.407654
4.086922	217.114220	5.412659
3.830189	211.045363	5.417664
4.505415	210.668403	5.422669
4.325781	220.130730	5.427674
4.138154	208.672847	5.432678
4.029388	214.802268	5.437683
4.117388	208.917014	5.442688
4.463629	201.966522	5.447693
4.382882	208.705333	5.452698
4.160873	211.938632	5.457702
4.331189	205.787468	5.462707
3.970422	208.659564	5.467712
4.129274	210.631364	5.472717
3.962276	211.989523	5.477722
3.776881	208.728403	5.482726
4.203514	215.011742	5.487731
4.078058	212.250642	5.492736
4.557577	209.752847	5.497741
4.205826	211.329593	5.502746
4.176183	210.059490	5.507750
4.309832	206.647459	5.512755
4.003258	210.998050	5.517760
4.562911	214.957515	5.522765
4.606427	219.291564	5.527770
4.466390	205.137141	5.532774
4.265135	204.412602	5.537779
4.564674	205.033749	5.542784
4.194055	205.721273	5.547789
4.325715	219.804731	5.552794
4.075039	219.432729	5.557798
5.054263	229.043654	5.562803
4.377518	219.278563	5.567808
4.662475	214.947648	5.572813
4.357964	214.096820	5.577818
4.266987	210.181934	5.582822
4.652952	210.042996	5.587827
4.513122	214.570102	5.592832
4.632391	209.233625	5.597837
4.589096	217.029606	5.602842
4.767988	216.473665	5.607846
4.583928	208.609175	5.612851
4.798652	211.920005	5.617856
4.236907	197.033998	5.622861
4.307357	214.875946	5.627866
4.809799	221.251885	5.632870
4.739967	226.546363	5.637875
4.433090	215.407593	5.642880
4.724699	218.371103	5.647885
4.659747	235.791238	5.652890
4.622479	230.890406	5.657894
5.082450	229.297303	5.662899
4.773015	228.421931	5.667904
4.628818	210.784930	5.672909
4.654676	225.327781	5.677914
4.548484	221.804396	5.682918
5.079364	224.948948	5.687923
4.803424	219.740437	5.692928
4.698447	208.421543	5.697933
4.849532	219.275018	5.702938
4.648186	218.945954	5.707942
4.983117	227.749214	5.712947
4.422093	223.436121	5.717952
4.867043	227.207808	5.722957
5.025103	231.837232	5.727962
5.069534	227.474162	5.732966
4.901079	225.523332	5.737971
4.699882	220.818865	5.742976
4.690634	226.825231	5.747981
4.880933	238.216766	5.752986
5.082663	234.471433	5.757990
5.291659	229.282327	5.762995
5.010157	236.270701	5.768000
5.163030	219.732694	5.773005
4.667508	219.598125	5.778010
4.793569	228.357977	5.783014
4.861219	232.488960	5.788019
4.961561	234.966571	5.793024
5.283091	236.669442	5.798029
5.122115	239.928043	5.803034
5.051296	234.750865	5.808038
5.285195	224.603547	5.813043
4.899320	235.417251	5.818048
5.089981	229.990559	5.823053
5.282551	234.051474	5.828058
5.300711	238.886175	5.833062
5.207769	229.675575	5.838067
4.731285	224.722908	5.843072
5.099901	223.020646	5.848077
5.100698	227.389822	5.853082
5.052279	228.482752	5.858086
5.304721	223.520997	5.863091
5.125814	239.253650	5.868096
5.362412	227.571520	5.873101
5.055759	237.009341	5.878106
5.169657	240.914830	5.883110
5.352321	230.025691	5.888115
4.993803	238.266223	5.893120
5.277389	231.743081	5.898125
5.305105	235.918246	5.903130
4.947320	238.188782	5.908134
5.315753	236.850371	5.913139
4.761376	247.136671	5.918144
5.111417	227.651035	5.923149
4.842663	237.038663	5.928154
5.056198	237.578292	5.933158
5.455138	246.039408	5.938163
5.607677	248.837918	5.943168
5.972265	243.175339	5.948173
5.701097	237.434580	5.953178
5.257390	230.227426	5.958182
5.244901	229.840484	5.963187
5.530188	241.802514	5.968192
5.452117	238.040634	5.973197
5.416799	233.528632	5.978202
5.720644	242.064662	5.983206
5.657914	239.376048	5.988211
5.410668	233.429090	5.993216
5.520915	240.128685	5.998221
5.335551	237.231379	6.003226
5.254758	238.484372	6.008230
5.262322	237.043963	6.013235
5.676833	249.555343	6.018240
5.946108	245.476795	6.023245
5.662495	241.234398	6.028250
5.677534	232.785252	6.033254
5.479516	230.734623	6.038259
5.331057	234.709432	6.043264
5.649140	231.075695	6.048269
5.330700	237.266243	6.053274
5.331813	232.207578	6.058278
5.358944	231.545553	6.063283
5.283478	236.091117	6.068288
5.486280	234.708893	6.073293
5.461556	243.770634	6.078298
5.415812	244.878968	6.083302
5.933125	251.771448	6.088307
5.601441	250.760337	6.093312
5.465272	234.017388	6.098317
5.104796	232.656427	6.103322
5.019926	245.065226	6.108326
5.468260	256.233104	6.113331
5.601748	266.235150	6.118336
6.315222	261.040255	6.123341
5.926861	250.429832	6.128346
5.444419	242.156211	6.133350
5.672518	236.527540	6.138355
5.339724	237.737513	6.143360
5.529733	237.907488	6.148365
5.308330	236.278106	6.153370
5.511557	235.547536	6.158374
5.598993	238.517530	6.163379
5.247702	238.097918	6.168384
5.184193	228.813134	6.173389
5.332428	232.710112	6.178394
5.276847	237.825208	6.183398
5.878812	241.284556	6.188403
5.746119	245.054436	6.193408
5.782452	239.936502	6.198413
5.959082	239.399894	6.203418
5.727619	240.293540	6.208422
5.952242	241.834332	6.213427
5.364233	242.346900	6.218432
5.403624	234.545682	6.223437
5.144133	230.986053	6.228442
5.326525	235.232046	6.233446
5.564098	241.127223	6.238451
5.449260	239.228154	6.243456
5.558982	233.674861	6.248461
5.690906	228.779323	6.253466
5.305852	222.284361	6.258470
5.644422	229.176189	6.263475
5.581913	232.697863	6.268480
5.826098	228.588424	6.273485
5.670262	230.150487	6.278490
5.682220	230.651898	6.283494
5.587465	223.779550	6.288499
5.821725	225.356804	6.293504
5.604397	217.506980	6.298509
5.889101	222.695638	6.303514
4.679568	214.626983	6.308518
5.123438	221.632124	6.313523
5.277988	236.284659	6.318528
5.492684	231.714748	6.323533
5.551266	230.807387	6.328538
5.387652	242.560906	6.333542
5.470741	237.701443	6.338547
5.317692	237.124418	6.343552
5.482139	230.695754	6.348557
5.394399	232.753405	6.353562
5.407889	234.482090	6.358566
5.341058	221.974028	6.363571
5.001301	231.746024	6.368576
5.936382	223.220072	6.373581
5.307036	229.803867	6.378586
5.563487	230.343140	6.383590
5.526843	231.703151	6.388595
5.171785	240.104493	6.393600
5.594631	237.659809	6.398605
5.646182	236.225206	6.403610
5.641016	230.632855	6.408614
5.510242	222.627187	6.413619
5.462725	242.085192	6.418624
5.400143	237.814710	6.423629
5.284394	239.455952	6.428634
5.282263	232.300265	6.433638
5.233214	226.284486	6.438643
4.836160	241.646154	6.443648
5.758054	245.115801	6.448653
5.686435	258.275504	6.453658
5.493859	253.708889	6.458662
5.534627	244.012400	6.463667
5.344100	248.866941	6.468672
5.260638	241.939045	6.473677
5.885876	247.773865	6.478682
5.662884	240.953113	6.483686
5.558042	234.085495	6.488691
5.313668	233.336031	6.493696
5.563738	236.337649	6.498701
5.237553	229.909447	6.503706
5.707305	238.796123	6.508710
5.831822	243.778778	6.513715
5.744846	233.149914	6.518720
5.589950	234.547319	6.523725
5.589517	231.722459	6.528730
5.549975	227.505339	6.533734
5.797335	230.134062	6.538739
5.676288	235.718085	6.543744
5.646448	230.980608	6.548749
5.887367	230.399190	6.553754
5.698787	235.006657	6.558758
5.785977	230.529363	6.563763
5.442714	233.579069	6.568768
5.518253	220.001661	6.573773
5.132463	233.004621	6.578778
5.203698	223.528022	6.583782
5.731818	224.040816	6.588787
5.642143	229.967958	6.593792
5.796706	232.794624	6.598797
5.497854	221.910859	6.603802
5.171493	222.056830	6.608806
5.645334	222.979863	6.613811
4.944942	229.394389	6.618816
5.308734	220.815020	6.623821
5.684806	227.375149	6.628826
5.199306	229.083450	6.633830
5.273537	232.498414	6.638835
5.139910	226.979848	6.643840
5.448121	227.852741	6.648845
5.600409	226.003829	6.653850
5.709439	236.639241	6.658854
6.009944	221.169720	6.663859
5.416219	230.541504	6.668864
5.356860	222.613300	6.673869
5.586794	229.838411	6.678874
5.743338	224.840967	6.683878
5.766885	219.759831	6.688883
5.079734	235.739288	6.693888
5.378859	229.893920	6.698893
5.455687	233.694451	6.703898
5.447240	225.869048	6.708902
5.646064	228.793223	6.713907
5.477154	228.180704	6.718912
5.457941	230.727548	6.723917
5.616095	226.587213	6.728922
5.354899	221.930051	6.733926
5.513398	227.828044	6.738931
5.140358	232.926128	6.743936
5.277179	233.471373	6.748941
5.570859	235.083668	6.753946
5.412962	229.610008	6.758950
5.873124	229.782214	6.763955
5.855614	232.572397	6.768960
5.640112	223.646632	6.773965
5.678085	225.118409	6.778970
5.525038	228.828181	6.783974
5.373063	232.325821	6.788979
5.118275	230.303012	6.793984
5.214385	231.373440	6.798989
5.659707	229.039152	6.803994
5.363099	230.189707	6.808998
5.914494	224.494885	6.814003
5.525594	234.489664	6.819008
5.472163	229.297126	6.824013
5.577787	231.296197	6.829018
5.635295	233.824769	6.834022
5.819640	225.153118	6.839027
5.404759	225.097740	6.844032
5.621086	224.988377	6.849037
4.988807	219.844838	6.854042
5.577962	228.750884	6.859046
5.491380	226.774651	6.864051
5.232550	236.056332	6.869056
5.340676	236.912923	6.874061
5.563096	228.694077	6.879066
5.203070	240.810362	6.884070
5.623053	233.576298	6.889075
5.509671	231.771914	6.894080
5.576808	238.645896	6.899085
5.559603	230.524468	6.904090
5.675804	231.326019	6.909094
5.866982	232.590449	6.914099
5.529246	231.238602	6.919104
5.698949	240.478874	6.924109
5.748427	235.893558	6.929114
5.442669	214.358733	6.934118
5.301858	216.557520	6.939123
5.387245	229.417516	6.944128
5.716260	229.239990	6.949133
5.442036	220.598610	6.954138
5.343395	221.069786	6.959142
5.654210	225.533058	6.964147
5.450115	227.912539	6.969152
5.459072	222.185117	6.974157
5.440638	221.030325	6.979162
5.436799	235.315222	6.984166
5.485497	234.864970	6.989171
5.339788	227.760113	6.994176
5.719950	229.358943	6.999181
5.942125	223.133261	7.004186
5.413224	220.232499	7.009190
5.110676	210.304750	7.014195
5.248750	229.370022	7.019200
5.611981	224.704222	7.024205
5.719335	221.742362	7.029210
5.706001	222.187601	7.034214
5.293309	214.320741	7.039219
4.855743	216.078524	7.044224
5.037281	221.387645	7.049229
5.491762	228.628413	7.054234
4.972400	229.826305	7.059238
5.507395	222.808452	7.064243
5.435807	233.759879	7.069248
5.483576	236.884741	7.074253
5.672017	228.174486	7.079258
5.520320	230.900142	7.084262
5.648339	226.947992	7.089267
5.160334	235.597816	7.094272
5.410152	231.161640	7.099277
5.527845	225.758965	7.104282
5.147126	223.255902	7.109286
5.632477	223.259674	7.114291
5.754144	228.578119	7.119296
5.684068	221.056537	7.124301
5.644066	220.335364	7.129306
5.512017	221.745029	7.134310
5.366366	230.619953	7.139315
5.655509	224.997599	7.144320
5.751707	220.528397	7.149325
5.900195	225.848993	7.154330
5.435104	232.442015	7.159334
5.698089	229.784945	7.164339
5.652098	224.518485	7.169344
5.850892	236.516125	7.174349
5.790175	222.077261	7.179354
5.123884	213.718386	7.184358
5.215587	211.372719	7.189363
5.310620	227.685957	7.194368
5.528683	228.825981	7.199373
5.615428	228.885487	7.204378
5.561064	225.774802	7.209382
5.571633	226.478906	7.214387
5.541963	225.907981	7.219392
5.760119	230.293934	7.224397
5.592922	215.526812	7.229402
5.190323	215.798545	7.234406
5.640245	211.128743	7.239411
5.224724	222.225458	7.244416
5.371165	224.344722	7.249421
5.587255	225.567308	7.254426
5.533285	228.534007	7.259430
5.678183	226.442642	7.264435
5.409798	229.085227	7.269440
5.514749	221.485774	7.274445
5.417841	216.559431	7.279450
5.314097	222.944332	7.284454
5.323286	222.974786	7.289459
5.362186	224.525510	7.294464
5.336590	226.962618	7.299469
5.574128	218.121340	7.304474
5.648144	221.536336	7.309478
5.745638	223.701184	7.314483
5.933335	217.768768	7.319488
5.288948	217.527666	7.324493
5.448391	224.542292	7.329498
5.474294	225.047859	7.334502
5.874204	218.908399	7.339507
5.226871	217.908471	7.344512
5.221410	208.402693	7.349517
5.631389	216.884222	7.354522
5.475578	225.264026	7.359526
5.774720	217.669141	7.364531
5.512204	214.366244	7.369536
5.390478	211.009791	7.374541
5.188851	217.251746	7.379546
5.366774	224.855104	7.384550
5.653152	225.193570	7.389555
5.482393	237.505007	7.394560
5.534208	230.818638	7.399565
5.893524	223.040379	7.404570
5.493877	225.991297	7.409574
5.433541	209.290347	7.414579
5.293736	207.543861	7.419584
5.264065	211.696319	7.424589
5.573534	223.142055	7.429594
5.642714	228.076375	7.434598
5.981008	215.350221	7.439603
5.149071	217.273807	7.444608
4.897511	211.586950	7.449613
5.481964	219.164975	7.454618
5.148046	224.342385	7.459622
5.633443	220.391541	7.464627
5.545618	231.845357	7.469632
5.559094	238.322742	7.474637
5.772816	227.115564	7.479642
5.771652	224.249691	7.484646
5.558224	215.684268	7.489651
5.077859	214.417903	7.494656
5.596394	226.802342	7.499661
5.729607	224.693815	7.504666
5.500996	229.541625	7.509670
5.767606	232.720997	7.514675
5.309883	228.872700	7.519680
5.279378	209.585536	7.524685
5.200242	221.471417	7.529690
5.578774	222.466236	7.534694
5.898712	225.207043	7.539699
5.604388	226.727393	7.544704
5.506705	215.410523	7.549709
5.661158	216.310519	7.554714
5.523005	218.341216	7.559718
5.613277	213.063035	7.564723
5.413611	215.811975	7.569728
5.057812	206.386055	7.574733
5.653267	209.985612	7.579738
5.414331	217.887983	7.584742
5.870192	213.356457	7.589747
5.436130	210.466240	7.594752
5.235967	203.050339	7.599757
5.443806	206.397041	7.604762
5.586730	220.700204	7.609766
5.847140	202.592099	7.614771
5.640339	214.890150	7.619776
5.411573	203.954356	7.624781
5.536936	207.244299	7.629786
5.312395	200.733844	7.634790
5.508283	200.732065	7.639795
5.274016	211.743608	7.644800
5.337968	207.820420	7.649805
5.466815	215.086573	7.654810
5.550267	218.082492	7.659814
5.439033	215.844350	7.664819
5.673775	216.026343	7.669824
5.605865	212.971552	7.674829
5.647998	213.847907	7.679834
5.410358	214.008538	7.684838
5.537227	205.918472	7.689843
5.236650	210.502241	7.694848
5.171361	214.435624	7.699853
5.783890	211.353983	7.704858
5.380273	221.816108	7.709862
5.140870	224.001773	7.714867
5.787143	226.603187	7.719872
5.754231	224.362340	7.724877
5.516706	216.996542	7.729882
5.653814	217.396212	7.734886
5.484706	209.453465	7.739891
5.213743	213.390397	7.744896
4.781509	220.579399	7.749901
5.603046	228.633031	7.754906
5.563371	243.996005	7.759910
5.715061	239.477030	7.764915
5.822973	240.118524	7.769920
5.754610	234.105749	7.774925
5.539026	218.909569	7.779930
5.113201	218.213667	7.784934
5.388778	209.894806	7.789939
5.474826	220.790045	7.794944
5.456644	235.222704	7.799949
5.364659	228.818148	7.804954
5.526480	231.934743	7.809958
5.793699	217.375223	7.814963
5.726657	218.161012	7.819968
5.570124	207.384808	7.824973
5.717104	208.855430	7.829978
5.311459	203.847449	7.834982
5.673792	209.988940	7.839987
5.512485	213.911962	7.844992
5.244947	214.431581	7.849997
5.656103	208.970565	7.855002
5.096700	213.003025	7.860006
5.379494	204.629260	7.865011
5.501903	208.890913	7.870016
5.300058	214.924098	7.875021
5.649318	212.664878	7.880026
5.522803	220.818660	7.885030
6.001356	213.819089	7.890035
5.450058	210.222642	7.895040
5.179183	207.974555	7.900045
5.232502	201.715061	7.905050
5.464510	215.947404	7.910054
5.690089	216.431373	7.915059
5.433984	211.251414	7.920064
5.312247	213.924947	7.925069
5.655248	209.591324	7.930074
5.520185	217.673671	7.935078
5.670453	209.133880	7.940083
5.441146	211.726087	7.945088
5.176296	207.085317	7.950093
5.448622	214.711937	7.955098
5.730569	235.067743	7.960102
5.676518	224.035133	7.965107
5.349530	217.711462	7.970112
5.301730	208.984216	7.975117
5.696059	211.643837	7.980122
5.270046	227.033568	7.985139
5.960992	220.473001	7.990157
5.530651	218.798352	7.995174
5.276091	214.432994	8.000192
5.411570	212.484068	8.005210
5.653979	215.627433	8.010227
5.537484	211.657121	8.015245
5.541508	215.781132	8.020262
5.312095	215.485759	8.025280
5.655116	215.382109	8.030298
5.455312	225.640818	8.035315
5.722372	217.366482	8.040333
5.549830	218.475970	8.045350
5.434164	215.417502	8.050368
5.784800	219.560126	8.055386
5.252800	217.876059	8.060403
5.566709	228.269368	8.065421
5.580469	229.614922	8.070438
5.638646	223.244387	8.075456
5.870464	223.385256	8.080474
5.498032	224.680492	8.085491
5.469637	217.875341	8.090509
5.610837	217.752625	8.095526
5.500882	232.165917	8.100544
5.660866	229.364312	8.105562
5.524117	234.441151	8.110579
5.788913	230.906902	8.115597
5.836378	232.262986	8.120614
5.527535	218.745322	8.125632
5.491615	223.781215	8.130650
5.527036	234.028550	8.135667
5.495883	235.523100	8.140685
5.840749	237.722765	8.145702
5.752112	231.116325	8.150720
6.157472	227.692727	8.155738
5.492063	220.365099	8.160755
5.658630	207.606506	8.165773
5.436717	213.283544	8.170790
5.607715	221.414434	8.175808
6.193486	221.661130	8.180826
5.713785	225.175688	8.185843
5.448677	210.013456	8.190861
5.511082	219.158427	8.195878
5.441986	228.263920	8.200896
5.728344	226.124253	8.205914
5.683710	230.180108	8.210931
5.835824	226.423576	8.215949
5.867606	221.262598	8.220966
5.576774	231.008494	8.225984
5.877594	228.626748	8.231002
6.153149	235.251914	8.236019
5.694716	226.408918	8.241037
5.895835	226.949019	8.246054
5.756048	219.479597	8.251072
5.862542	212.574555	8.256090
5.581687	219.491462	8.261107
5.449034	218.729770	8.266125
6.328689	220.435939	8.271142
6.276769	219.800525	8.276160
5.737136	202.131304	8.281178
5.267254	210.409306	8.286195
5.470704	215.275392	8.291213
5.935998	221.684830	8.296230
6.133478	231.856441	8.301248
5.837796	220.053383	8.306266
5.838765	223.439457	8.311283
5.769721	214.889268	8.316301
6.087617	209.175692	8.321318
5.441829	222.747809	8.326336
5.958085	225.258439	8.331354
5.892668	227.433626	8.336371
5.823597	220.647429	8.341389
5.941155	226.501976	8.346406
5.893540	231.170484	8.351424
5.821501	223.901939	8.356442
5.985312	235.918520	8.361459
5.845786	227.499213	8.366477
5.704519	223.419153	8.371494
5.633781	231.098565	8.376512
5.931943	233.176121	8.381530
6.222617	239.956716	8.386547
5.634699	233.244985	8.391565
6.006171	228.892600	8.396582
6.132943	228.519681	8.401600
6.240531	221.996295	8.406618
5.784311	223.708495	8.411635
5.824778	223.648797	8.416653
5.995163	233.862496	8.421670
5.948785	231.560052	8.426688
6.041467	233.016387	8.431706
6.099683	233.846966	8.436723
5.827306	227.871858	8.441741
5.944281	226.118304	8.446758
5.716863	233.601218	8.451776
5.844933	237.052706	8.456794
5.880820	234.169442	8.461811
5.879867	235.192259	8.466829
5.977621	236.136595	8.471846
6.027836	233.276345	8.476864
6.424720	225.616072	8.481882
6.424529	228.323869	8.486899
6.017076	231.596819	8.491917
6.296591	224.096823	8.496934
5.733066	221.893832	8.501952
6.212114	222.198168	8.506970
6.334274	232.334172	8.511987
5.880588	226.623966	8.517005
5.968408	221.110300	8.522022
5.820420	227.047215	8.527040
6.018428	223.106824	8.532058
6.456244	235.888581	8.537075
5.904824	232.162696	8.542093
6.025507	215.501431	8.547110
6.025700	233.280394	8.552128
6.078771	228.561041	8.557146
6.127126	231.346482	8.562163
5.924096	235.430155	8.567181
6.027455	227.089789	8.572199
6.158435	230.499800	8.577216
6.088593	234.032592	8.582234
6.214461	233.969064	8.587251
6.122544	241.629689	8.592269
6.286414	231.910361	8.597287
6.106138	241.639050	8.602304
6.320849	228.478494	8.607322
5.834039	234.010600	8.612339
5.887710	231.730446	8.617357
5.892127	222.225286	8.622375
6.178225	233.235118	8.627392
5.886000	230.358762	8.632410
6.076403	222.579168	8.637427
6.015446	233.169692	8.642445
6.285036	229.038285	8.647463
6.414746	244.834300	8.652480
6.444512	234.501571	8.657498
6.365353	236.334935	8.662515
6.317959	239.491870	8.667533
6.394618	239.391825	8.672551
6.116807	232.511899	8.677568
6.283674	232.211628	8.682586
6.066729	234.801704	8.687603
6.500615	238.962927	8.692621
6.533873	235.130230	8.697639
6.175712	237.846429	8.702656
6.261124	232.011262	8.707674
6.343268	225.223609	8.712691
6.086946	232.512219	8.717709
6.171918	227.772122	8.722727
6.588372	234.908650	8.727744
5.993556	239.851695	8.732762
6.155747	236.058880	8.737779
6.044291	240.847778	8.742797
6.425523	232.385256	8.747815
6.485830	241.659946	8.752832
6.199692	228.747773	8.757850
6.056077	241.563260	8.762867
6.099209	245.807413	8.767885
6.151565	224.966113	8.772903
6.015369	230.863326	8.777920
6.260318	234.277683	8.782938
6.667299	242.166726	8.787955
6.494035	242.364353	8.792973
6.443207	229.914131	8.797991
6.218923	230.059746	8.803008
6.532036	237.338589	8.808026
6.366722	226.130575	8.813043
6.210236	229.159335	8.818061
6.148693	216.521453	8.823079
6.442623	238.192896	8.828096
6.577246	242.665786	8.833114
6.508295	237.353239	8.838131
6.485336	246.429469	8.843149
6.266114	236.665649	8.848167
6.444177	238.370608	8.853184
6.600249	248.744325	8.858202
6.717158	234.494524	8.863219
6.308608	240.604548	8.868237
6.194547	234.547988	8.873255
6.480951	234.459465	8.878272
6.582596	248.596842	8.883290
6.499052	243.362300	8.888307
6.408452	245.389940	8.893325
6.543914	237.483203	8.898343
6.687219	242.140922	8.903360
6.810018	241.367858	8.908378
6.429578	225.715514	8.913395
5.967018	224.055347	8.918413
6.177822	229.623994	8.923431
6.870165	248.525898	8.928448
7.012647	248.623876	8.933466
6.430029	232.592773	8.938483
6.473521	242.965081	8.943501
6.964790	238.095454	8.948519
6.736870	241.230007	8.953536
6.404445	230.357259	8.958554
6.607683	225.374700	8.963571
6.630391	229.372735	8.968589
6.382845	229.383124	8.973607
6.488870	228.981879	8.978624
6.227492	233.541667	8.983642
6.700945	237.333833	8.988659
6.679293	253.642544	8.993677
7.152648	246.074491	8.998695
6.600391	236.526616	9.003712
6.345509	241.792254	9.008730
6.392723	230.166161	9.013747
6.574446	246.168662	9.018765
6.747058	256.852215	9.023783
7.062872	246.528587	9.028800
6.514572	240.198827	9.033818
6.507715	236.334509	9.038835
6.142360	242.093845	9.043853
6.796743	247.877440	9.048871
6.887123	249.659165	9.053888
6.499513	251.985498	9.058906
6.533286	243.696982	9.063923
6.399251	250.837180	9.068941
6.582769	252.547602	9.073959
6.820501	258.626432	9.078976
6.464520	258.050980	9.083994
6.723777	254.467098	9.089011
6.434618	249.737911	9.094029
6.691461	258.688537	9.099047
6.774518	252.213139	9.104064
6.526137	257.745997	9.109082
6.686297	251.381663	9.114099
6.719355	261.004568	9.119117
6.684310	257.441263	9.124135
7.009186	256.176014	9.129152
6.838323	262.914875	9.134170
6.770234	259.517651	9.139187
6.925789	256.584195	9.144205
6.677934	249.721687	9.149223
7.008535	256.054285	9.154240
6.781063	258.081147	9.159258
6.673068	252.307642	9.164275
6.482933	262.489132	9.169293
6.725638	259.905003	9.174311
6.902921	253.326576	9.179328
6.876892	255.915331	9.184346
6.924110	256.482550	9.189363
6.829914	259.495306	9.194381
6.936972	252.747942	9.199399
6.881377	256.038693	9.204416
7.019616	253.492920	9.209434
6.965491	258.124582	9.214451
6.964752	261.072296	9.219469
6.855602	257.179721	9.224487
7.036840	261.740027	9.229504
7.142272	261.670214	9.234522
7.200445	255.949727	9.239539
6.886272	258.012177	9.244557
7.053470	255.979417	9.249575
7.115401	249.592510	9.254592
6.891794	265.077502	9.259610
7.137334	254.042173	9.264627
7.193197	257.224058	9.269645
7.125624	257.503054	9.274663
7.276882	254.816406	9.279680
7.062490	260.646913	9.284698
7.294870	253.671766	9.289715
7.279782	258.565578	9.294733
6.951267	241.582930	9.299751
6.818274	241.285166	9.304768
6.837107	252.819432	9.309786
7.181495	263.040768	9.314803
6.783994	264.172661	9.319821
6.473038	263.441885	9.324839
7.265547	261.371722	9.329856
6.896159	260.640576	9.334874
7.351658	256.253012	9.339891
6.945304	253.473312	9.344909
6.980564	263.827980	9.349927
6.845111	261.387931	9.354944
6.920839	263.579014	9.359962
6.965545	258.895667	9.364979
6.874901	257.587822	9.369997
6.892833	264.502404	9.375015
7.295627	257.652192	9.380032
7.074608	259.185773	9.385050
7.120009	264.669737	9.390067
6.901462	261.472653	9.395085
6.796393	260.978048	9.400103
6.901772	258.443702	9.405120
6.799382	266.500420	9.410138
7.376375	261.409169	9.415155
7.284814	257.867285	9.420173
7.110881	259.188419	9.425191
7.357300	256.455398	9.430208
7.129037	264.556959	9.435226
7.283683	251.456227	9.440243
7.126385	262.099636	9.445261
6.793216	257.850643	9.450279
7.163438	259.424705	9.455296
7.354316	277.880884	9.460314
6.953633	266.113077	9.465331
7.785028	274.027568	9.470349
7.413710	272.018694	9.475367
7.423394	267.605870	9.480384
7.326326	265.232423	9.485402
7.248790	267.671418	9.490419
7.294860	260.261399	9.495437
7.128897	261.480313	9.500455
7.080210	257.161782	9.505472
7.119988	261.049875	9.510490
7.196810	260.410193	9.515507
7.259840	258.033910	9.520525
7.122374	262.615436	9.525543
7.357982	261.171592	9.530560
7.401227	267.757206	9.535578
7.255584	267.291008	9.540595
7.464655	270.335438	9.545613
7.426880	261.742491	9.550631
7.782977	254.113801	9.555648
7.655715	253.912969	9.560666
7.519414	258.519558	9.565683
7.662814	253.142388	9.570701
7.614568	260.998181	9.575719
7.377095	257.340168	9.580736
7.516935	266.362660	9.585754
7.533410	259.282279	9.590771
7.722356	250.994844	9.595789
7.370470	261.277252	9.600807
7.604177	264.276823	9.605824
7.559795	263.548720	9.610842
7.328549	256.639445	9.615859
7.292367	258.560790	9.620877
7.387559	265.270850	9.625895
7.235146	255.657555	9.630912
7.246247	260.181237	9.635930
7.182828	260.071445	9.640947
7.195954	263.970000	9.645965
7.191732	261.042487	9.650983
7.381681	261.451792	9.656000
7.434746	256.315890	9.661018
7.368851	259.658735	9.666035
7.367359	262.616034	9.671053
7.269335	261.940462	9.676071
7.295788	250.958181	9.681088
7.606367	269.727054	9.686106
7.854637	271.638823	9.691123
7.513237	266.084681	9.696141
7.451093	261.711442	9.701159
7.697977	257.406849	9.706176
7.473103	263.866958	9.711194
7.374267	268.240511	9.716211
7.515073	258.635206	9.721229
7.609882	266.755890	9.726247
7.726601	267.867679	9.731264
7.391616	266.178178	9.736282
7.691018	268.561641	9.741299
7.583891	261.907578	9.746317
7.461646	264.299888	9.751335
7.849127	264.533280	9.756352
7.710572	276.858882	9.761370
7.519661	268.472801	9.766387
7.613821	261.623307	9.771405
7.586827	262.075856	9.776423
7.965934	265.788049	9.781440
7.763277	266.125945	9.786458
7.281374	263.550499	9.791475
7.607427	266.781831	9.796493
8.094375	284.683864	9.801511
7.815977	269.343779	9.806528
7.576338	263.811661	9.811546
7.508796	264.882714	9.816563
7.704685	266.468143	9.821581
7.250432	267.451091	9.826599
7.811490	282.245916	9.831616
8.141312	284.148145	9.836634
7.769528	285.424350	9.841651
7.812783	268.232323	9.846669
7.759192	261.093426	9.851687
7.596278	261.778565	9.856704
7.814399	267.484932	9.861722
7.892991	275.721748	9.866739
7.714934	257.892040	9.871757
7.739824	267.371061	9.876775
8.011820	267.849638	9.881792
7.746207	257.332524	9.886810
7.722675	270.552189	9.891827
7.997907	274.403626	9.896845
7.834712	268.588220	9.901863
7.842740	261.493375	9.906880
7.572073	262.368849	9.911898
7.832117	272.196247	9.916915
8.180749	261.734964	9.921933
7.728394	274.544899	9.926951
8.028717	269.951131	9.931968
7.913746	263.572829	9.936986
7.586756	266.867970	9.942003
8.086045	270.574074	9.947021
7.910632	274.211668	9.952039
8.013445	274.457825	9.957056
7.928953	260.630659	9.962074
7.929191	266.547664	9.967091
7.816678	259.534700	9.972109
7.952848	264.553278	9.977127
8.080484	266.733123	9.982144
8.035829	271.688343	9.987162
7.833118	265.282678	9.992179
7.950625	270.600792	9.997197
7.954531	282.023798	10.002215
7.816288	278.312463	10.007232
8.093189	271.977280	10.012250
7.941871	279.650325	10.017267
8.314331	275.253596	10.022285
7.901172	273.238614	10.027303
8.306686	271.225548	10.032320
8.147033	262.392815	10.037338
7.853684	263.041461	10.042355
7.874873	260.018478	10.047373
7.914460	277.131826	10.052391
8.087328	265.684951	10.057408
8.396258	275.555230	10.062426
7.773493	268.968825	10.067443
8.236806	273.141252	10.072461
8.193579	269.888470	10.077479
8.011356	265.742197	10.082496
8.336827	262.435167	10.087514
7.961975	264.923608	10.092531
7.935560	264.003370	10.097549
8.303024	278.803089	10.102567
8.063609	272.393669	10.107584
8.063072	265.521050	10.112602
8.294865	270.852926	10.117619
8.286174	267.231869	10.122637
7.811566	260.123812	10.127655
8.079368	267.062604	10.132672
8.357224	271.017767	10.137690
8.151334	269.901424	10.142707
8.065280	265.191100	10.147725
7.903474	281.852998	10.152743
8.114476	273.760924	10.157760
8.361909	274.994365	10.162778
8.006397	279.682424	10.167795
8.488372	272.002571	10.172813
8.118232	275.982891	10.177831
8.375416	269.486686	10.182848
8.330036	275.461287	10.187866
8.296270	273.832178	10.192883
8.555045	267.793292	10.197901
8.724091	274.053226	10.202919
8.275400	274.394717	10.207936
8.511841	266.579536	10.212954
8.061743	267.596549	10.217971
8.314591	271.912192	10.222989
8.470733	269.732837	10.228007
8.275509	271.256091	10.233024
8.350037	263.005400	10.238042
8.532421	275.549260	10.243059
8.258003	265.090314	10.248077
8.050925	266.779506	10.253095
8.505965	267.807063	10.258112
8.516318	273.186039	10.263130
8.297103	280.740275	10.268147
8.539011	281.466521	10.273165
8.500911	267.531146	10.278183
8.299293	260.651968	10.283200
8.575584	269.022092	10.288218
8.094929	273.792747	10.293235
8.168261	271.572639	10.298253
8.360801	278.359061	10.303271
8.208392	273.229901	10.308288
8.404556	266.774754	10.313306
8.093933	271.793474	10.318323
8.675526	272.918086	10.323341
8.709779	270.306454	10.328359
8.117046	274.283563	10.333376
8.549260	274.948622	10.338394
8.361365	281.289377	10.343411
8.677737	274.563061	10.348429
8.483233	280.210607	10.353447
8.539210	275.673816	10.358464
8.552263	280.361292	10.363482
8.773558	289.781346	10.368499
8.713858	282.873752	10.373517
8.568096	282.215079	10.378535
8.474712	273.971592	10.383552
8.347475	269.223500	10.388570
8.631766	280.429291	10.393587
8.674403	271.751240	10.398605
8.590754	282.348482	10.403623
8.380391	272.412859	10.408640
8.502184	267.231542	10.413658
8.379013	279.822979	10.418675
8.505526	275.474010	10.423693
8.658931	281.553355	10.428711
8.752305	284.410686	10.433728
8.781774	277.239916	10.438746
8.538354	282.263954	10.443763
8.736813	268.436906	10.448781
8.637227	279.876024	10.453799
8.867412	281.146862	10.458816
8.912954	278.858501	10.463834
8.658026	287.421790	10.468851
8.595340	279.637398	10.473869
8.500336	278.058846	10.478887
8.600763	273.231128	10.483904
8.622998	276.247848	10.488922
8.438879	275.251184	10.493939
8.584130	276.876053	10.498957
9.009046	293.850533	10.503975
8.740629	284.015455	10.508992
8.862749	279.679792	10.514010
8.736394	291.359757	10.519027
8.879965	291.852019	10.524045
9.033341	281.720910	10.529063
8.799280	279.371946	10.534080
8.756247	280.010019	10.539098
8.747811	286.152431	10.544115
8.962698	286.128689	10.549133
9.073536	279.099876	10.554151
8.677837	279.619298	10.559168
8.773126	276.505885	10.564186
8.651566	276.884801	10.569203
9.151400	283.358307	10.574221
9.184743	282.138447	10.579239
8.562943	280.894365	10.584256
9.050778	286.965821	10.589274
8.843253	282.697259	10.594291
8.602492	286.685839	10.599309
9.110981	278.203481	10.604327
9.247787	293.080148	10.609344
8.983976	284.093217	10.614362
8.937670	281.005004	10.619379
8.782210	277.053367	10.624397
9.045016	281.146568	10.629415
9.047327	286.769784	10.634432
9.163132	285.858959	10.639450
8.599209	284.653200	10.644467
8.977556	290.959442	10.649485
9.120607	301.265793	10.654503
9.143554	299.435359	10.659520
9.332799	295.903392	10.664538
9.081815	288.015777	10.669555
8.823001	279.308922	10.674573
8.961934	282.869175	10.679591
8.934568	289.200718	10.684608
9.352151	288.523758	10.689626
8.973064	293.486875	10.694643
9.274031	299.593741	10.699661
9.520611	295.686795	10.704679
9.148074	286.906129	10.709696
9.021822	275.051410	10.714714
8.746124	282.989960	10.719731
8.867805	291.945869	10.724749
9.532606	296.812726	10.729767
9.562540	287.215201	10.734784
9.103161	281.108254	10.739802
9.213339	270.904987	10.744819
8.799976	279.139509	10.749837
9.290592	274.942122	10.754855
9.129640	289.893546	10.759872
9.322561	281.151068	10.764890
9.266611	288.361169	10.769907
8.981539	286.793276	10.774925
9.163721	293.107972	10.779943
9.121803	298.365714	10.784960
9.334549	293.208095	10.789978
9.275240	293.223889	10.794995
9.375145	294.148959	10.800013
9.236523	293.763713	10.805031
9.159395	293.674990	10.810048
9.068991	285.462590	10.815066
9.553908	292.878800	10.820083
9.484423	295.480637	10.825101
9.594545	292.667852	10.830119
9.246998	305.395222	10.835136
9.396029	296.249339	10.840154
9.477714	292.308110	10.845171
9.429084	289.586311	10.850189
9.298528	276.921263	10.855207
9.347859	294.023644	10.860224
9.260074	289.777461	10.865242
9.470716	290.110965	10.870259
9.132133	294.114776	10.875277
9.375758	287.983574	10.880295
9.486206	289.654886	10.885312
9.739272	289.899739	10.890330
9.648939	285.398348	10.895347
9.227380	282.841904	10.900365
9.376948	283.538348	10.905383
9.457173	292.147281	10.910400
9.329230	286.029752	10.915418
9.236925	295.318764	10.920435
9.459147	296.250035	10.925453
9.736813	289.671743	10.930471
9.464224	288.180797	10.935488
9.623603	288.304544	10.940506
9.457248	286.453094	10.945523
9.307499	296.764007	10.950541
9.783204	286.431240	10.955559
9.534994	290.118040	10.960576
9.633692	289.178322	10.965594
9.668838	290.558418	10.970611
9.408391	290.681263	10.975629
9.623117	287.770145	10.980647
9.807499	296.107258	10.985664
9.590928	293.020307	10.990682
9.444833	286.605820	10.995699
9.366984	292.878955	11.000717
9.583391	290.030688	11.005735
9.242194	294.767012	11.010752
9.359715	294.064191	11.015770
9.359472	295.165791	11.020787
9.018450	290.776009	11.025805
10.129852	294.964295	11.030823
9.599516	302.989835	11.035840
10.120466	296.345262	11.040858
9.652888	295.503178	11.045875
9.474522	294.341524	11.050893
9.562784	284.308909	11.055911
9.728396	296.580857	11.060928
9.697822	305.263849	11.065946
10.109056	306.370808	11.070963
10.068679	313.468048	11.075981
9.847542	289.548334	11.080999
9.925380	297.580161	11.086016
9.826698	290.514541	11.091034
9.798226	288.572199	11.096051
9.560119	297.735599	11.101069
9.832501	288.671494	11.106087
9.409281	294.357810	11.111104
9.859341	304.067284	11.116122
10.284214	301.656747	11.121139
10.000554	304.112061	11.126157
9.948037	290.115800	11.131175
9.658514	286.961319	11.136192
9.761130	289.956059	11.141210
9.689719	285.066735	11.146227
9.989651	294.102183	11.151245
10.220769	300.144190	11.156263
9.661319	294.911150	11.161280
10.049192	289.445415	11.166298
10.256232	292.275582	11.171315
9.656422	292.848874	11.176333
9.851051	286.469694	11.181351
10.316976	292.916927	11.186368
10.026119	292.217732	11.191386
9.877886	280.874487	11.196403
9.663240	294.698250	11.201421
10.255938	298.020608	11.206439
10.079981	301.244905	11.211456
10.107355	298.479714	11.216474
9.999704	301.646042	11.221491
9.924285	298.350932	11.226509
9.923404	302.226431	11.231527
10.507710	307.563390	11.236544
9.965537	292.602007	11.241562
10.129356	289.840818	11.246579
9.872876	300.862590	11.251597
10.403317	299.208746	11.256615
10.101127	307.687889	11.261632
9.914716	298.004129	11.266650
10.238352	302.008973	11.271667
10.205903	318.723345	11.276685
10.524865	305.966200	11.281703
9.974884	290.567401	11.286720
9.598487	296.782885	11.291738
10.203316	302.381720	11.296755
10.358809	310.492976	11.301773
10.268276	311.100578	11.306791
10.460506	306.952797	11.311808
10.499623	309.809112	11.316826
10.280842	290.379495	11.321843
10.014092	300.752806	11.326861
10.242193	294.422058	11.331879
10.343937	307.723225	11.336896
10.272372	312.988743	11.341914
10.581600	299.794484	11.346931
10.086416	298.940919	11.351949
10.092048	296.210670	11.356967
10.509665	304.243244	11.361984
10.522462	307.517045	11.367002
10.401316	297.220398	11.372019
10.008656	307.922568	11.377037
10.422964	303.096462	11.382055
10.634289	308.273755	11.387072
10.225490	302.881565	11.392090
10.448834	298.574315	11.397107
10.253155	308.494777	11.402125
10.230362	303.970242	11.407143
10.403322	304.757713	11.412160
9.743964	315.911645	11.417178
10.513062	308.887623	11.422195
10.300516	309.094523	11.427213
10.257064	302.436842	11.432231
10.507546	300.574137	11.437248
10.286608	306.219495	11.442266
10.431550	305.897391	11.447283
10.455508	304.183557	11.452301
10.239683	304.955825	11.457319
10.314682	292.126227	11.462336
10.029165	304.288548	11.467354
10.506126	307.714130	11.472371
10.698767	310.448718	11.477389
10.670323	313.372354	11.482407
11.015389	310.478807	11.487424
10.372135	309.541004	11.492442
10.374891	292.014451	11.497459
10.257813	305.901922	11.502477
11.032767	313.923043	11.507495
10.857304	305.244221	11.512512
10.612490	297.854231	11.517530
10.605684	304.804237	11.522547
10.536569	296.392868	11.527565
10.572285	301.556477	11.532583
10.660162	303.852965	11.537600
10.353135	294.396257	11.542618
11.253218	305.364184	11.547635
10.475342	299.704429	11.552653
10.295590	295.535675	11.557671
11.169350	310.136678	11.562688
10.910582	311.606716	11.567706
10.718810	304.508250	11.572723
10.628273	295.705763	11.577741
10.632115	295.699101	11.582759
10.627900	299.821258	11.587776
10.751643	319.209377	11.592794
11.322715	311.850132	11.597811
10.829119	307.818598	11.602829
10.429451	311.131373	11.607847
11.138489	311.223187	11.612864
10.668282	307.285836	11.617882
10.871008	300.981125	11.622899
10.795716	303.640670	11.627917
10.738535	310.743681	11.632935
11.319779	315.147052	11.637952
11.158856	311.202569	11.642970
11.024059	307.017346	11.647987
10.776044	304.105694	11.653005
10.762154	296.540902	11.658023
11.120393	293.414946	11.663040
10.942516	299.407029	11.668058
10.791600	292.359008	11.673075
10.787945	295.146245	11.678093
10.857691	300.099440	11.683111
10.992874	303.029155	11.688128
11.236840	322.117707	11.693146
10.836367	303.710389	11.698163
11.304923	314.745509	11.703181
10.773419	313.544167	11.708199
10.983451	306.111757	11.713216
11.241925	319.300173	11.718234
11.245323	316.115858	11.723251
10.882176	307.598792	11.728269
10.958484	304.993230	11.733287
11.015237	308.537883	11.738304
11.266017	315.283695	11.743322
11.141667	308.824790	11.748339
10.907423	303.840899	11.753357
11.115619	322.982356	11.758375
11.440055	314.904158	11.763392
11.086281	318.462240	11.768410
11.113423	310.594425	11.773427
10.999399	315.377431	11.778445
10.838944	314.992429	11.783463
11.405320	320.237515	11.788480
11.276361	324.710441	11.793498
11.472177	314.247675	11.798515
11.168161	322.525150	11.803533
11.308030	325.712901	11.808551
11.488974	311.819122	11.813568
10.634482	308.067828	11.818586
10.741187	312.516681	11.823603
11.293059	318.944232	11.828621
11.010720	320.253848	11.833639
11.191473	321.081130	11.838656
10.938446	315.778285	11.843674
10.986378	312.135781	11.848691
11.183905	316.229687	11.853709
11.501608	319.048940	11.858727
11.376750	317.244672	11.863744
10.986478	320.385582	11.868762
11.358734	320.902196	11.873779
11.333520	324.857224	11.878797
11.543882	330.034673	11.883815
11.733754	326.751898	11.888832
11.549937	328.784594	11.893850
11.608564	312.741937	11.898867
11.876585	322.463985	11.903885
11.036602	325.435086	11.908903
11.646926	327.542942	11.913920
11.341880	317.331717	11.918938
11.235428	313.817386	11.923955
11.467401	317.940641	11.928973
11.321809	315.224467	11.933991
11.696014	320.193376	11.939008
11.465023	321.327749	11.944026
11.427989	313.820200	11.949043
12.079199	310.998901	11.954061
11.879604	327.250183	11.959079
11.734040	318.913819	11.964096
11.712524	319.539076	11.969114
11.660980	315.580718	11.974131
11.809028	319.108003	11.979149
11.947080	320.153361	11.984167
11.833638	316.277219	11.989184
11.616109	317.456830	11.994202
11.860421	320.659875	11.999219
11.479320	316.800162	12.004237
11.338659	320.277729	12.009255
11.758516	315.059457	12.014272
11.943175	320.919367	12.019290
11.659327	322.248151	12.024307
11.751800	318.349416	12.029325
11.696073	321.472951	12.034343
11.891879	320.234105	12.039360
11.844452	319.386560	12.044378
11.963448	319.374592	12.049395
12.007460	312.655955	12.054413
11.603478	308.755627	12.059431
11.829384	314.523910	12.064448
11.297825	320.492176	12.069466
11.539932	317.829242	12.074483
11.912493	315.811835	12.079501
11.563309	319.820458	12.084519
11.792676	312.031603	12.089536
11.786651	319.558974	12.094554
11.778331	318.834722	12.099571
12.123245	316.891043	12.104589
11.732800	324.869568	12.109607
11.984364	312.283848	12.114624
11.988093	320.207311	12.119642
12.187179	314.550067	12.124659
12.169883	319.791359	12.129677
11.642610	318.043434	12.134695
11.778785	318.773520	12.139712
11.421865	316.850757	12.144730
11.397059	320.632161	12.149747
11.975812	318.248153	12.154765
11.740831	328.648090	12.159783
12.073567	331.796347	12.164800
12.305463	330.507702	12.169818
11.909892	334.397325	12.174835
12.168909	323.388256	12.179853
12.139474	321.872071	12.184871
12.233627	321.034039	12.189888
12.381750	328.477456	12.194906
12.226282	338.022465	12.199923
12.225649	315.075033	12.204941
12.187942	319.401213	12.209959
11.788305	311.517799	12.214976
12.197099	314.300780	12.219994
12.246266	319.105713	12.225011
12.499808	322.042248	12.230029
12.178782	329.019097	12.235047
11.830768	319.130125	12.240064
11.787132	330.819326	12.245082
12.292432	333.864981	12.250099
12.465797	328.710328	12.255117
12.175406	335.205908	12.260135
12.331261	336.816510	12.265152
12.271562	338.466984	12.270170
12.239261	337.759087	12.275187
12.300618	330.810537	12.280205
12.456775	336.741157	12.285223
12.773603	330.399738	12.290240
12.700340	326.428980	12.295258
12.290167	328.058285	12.300275
12.382171	315.465850	12.305293
12.108568	322.630962	12.310311
12.552344	321.161014	12.315328
12.322004	317.353563	12.320346
12.236321	319.604496	12.325363
12.347660	322.919758	12.330381
12.074485	326.660942	12.335399
12.035610	335.035989	12.340416
12.290862	324.920550	12.345434
12.600910	320.577706	12.350451
12.815459	318.670103	12.355469
12.631014	329.876326	12.360487
12.876948	322.346806	12.365504
12.928238	325.687196	12.370522
12.296051	322.936335	12.375539
12.607819	317.296258	12.380557
12.493411	330.119884	12.385575
12.559391	325.057687	12.390592
12.471449	323.904042	12.395610
12.400667	330.169779	12.400627
12.763259	324.335605	12.405645
12.862655	335.699599	12.410663
12.521416	328.094248	12.415680
12.798029	338.613343	12.420698
12.769755	337.343115	12.425715
12.596914	323.416052	12.430733
12.084000	328.478906	12.435751
12.800744	325.581134	12.440768
13.043488	335.988742	12.445786
12.644207	336.379343	12.450803
12.727041	329.070863	12.455821
12.964135	334.083213	12.460839
12.709960	330.430941	12.465856
12.836601	331.610613	12.470874
12.810924	339.059005	12.475891
12.611851	332.861021	12.480909
12.422347	329.145034	12.485927
12.554944	337.032661	12.490944
12.698844	327.452083	12.495962
12.625337	333.816070	12.500979
12.733498	326.153372	12.505997
12.737442	337.715257	12.511015
12.704967	337.998257	12.516032
12.895450	331.354633	12.521050
12.564974	333.687859	12.526067
12.936818	327.113825	12.531085
12.842275	326.750116	12.536103
12.676780	330.449290	12.541120
12.768657	332.237101	12.546138
12.868612	332.638331	12.551155
13.363895	329.825528	12.556173
12.896974	334.291119	12.561191
12.784642	336.328464	12.566208
12.933472	331.657287	12.571226
12.906569	349.904465	12.576243
13.202495	343.629407	12.581261
13.161438	355.299290	12.586279
13.307478	338.656051	12.591296
13.366360	333.020630	12.596314
12.842678	326.652294	12.601331
12.932892	325.773852	12.606349
13.048957	331.196344	12.611367
13.066419	334.128615	12.616384
13.207736	326.290350	12.621402
13.073681	339.669278	12.626419
13.528465	334.808461	12.631437
13.237435	332.518850	12.636455
12.794162	326.930059	12.641472
13.218116	330.862489	12.646490
12.980238	347.908659	12.651507
13.798710	342.543114	12.656525
13.253802	334.319409	12.661543
12.953532	326.966442	12.666560
13.263972	322.484688	12.671578
13.249239	332.446415	12.676595
13.517862	349.315901	12.681613
13.256044	341.682400	12.686631
13.277493	337.283505	12.691648
13.275865	336.444607	12.696666
13.349460	337.982814	12.701683
13.379226	341.992399	12.706701
13.558352	339.443403	12.711719
13.418469	335.795424	12.716736
13.576640	327.853554	12.721754
12.887672	327.790667	12.726771
13.253392	327.686639	12.731789
13.650293	339.922606	12.736807
13.592444	350.500094	12.741824
14.063933	340.912683	12.746842
13.300179	335.026666	12.751859
13.227243	330.617224	12.756877
13.396880	332.705336	12.761895
13.251269	342.867316	12.766912
13.547363	338.611843	12.771930
13.627399	341.395524	12.776947
13.763402	337.549964	12.781965
14.092351	341.216337	12.786983
13.674118	340.552750	12.792000
13.699843	313.902808	12.797018
13.192162	319.195206	12.802035
13.325665	318.423627	12.807053
13.162222	331.289600	12.812071
13.456260	330.717076	12.817088
13.747427	342.095396	12.822106
13.708138	339.952772	12.827123
13.724071	345.302501	12.832141
13.710310	335.553971	12.837159
13.417298	344.719632	12.842176
13.921881	341.716042	12.847194
14.013915	334.415594	12.852211
13.869568	339.695607	12.857229
13.930000	330.102778	12.862247
13.708547	332.062443	12.867264
13.978908	336.896055	12.872282
13.672700	340.774922	12.877299
13.682010	332.827826	12.882317
13.901283	338.811733	12.887335
13.605204	337.201370	12.892352
13.676324	338.339196	12.897370
13.504528	334.304887	12.902387
13.578228	334.350462	12.907405
14.021722	332.378811	12.912423
13.846458	329.932328	12.917440
14.061058	336.484976	12.922458
13.707488	339.626486	12.927475
13.437084	339.962309	12.932493
14.067838	340.391343	12.937511
13.712891	336.656934	12.942528
13.845041	335.166080	12.947546
14.101197	336.088914	12.952563
14.081315	337.941461	12.957581
13.995935	340.012478	12.962599
13.905754	341.623519	12.967616
14.111370	331.686209	12.972634
13.972676	341.926003	12.977651
13.738933	337.431148	12.982669
14.364859	343.023556	12.987687
14.373132	349.567310	12.992704
14.111703	340.725139	12.997722
14.302474	341.213209	13.002739
14.053200	334.177330	13.007757
14.031430	327.175456	13.012775
13.962058	343.248695	13.017792
14.066500	356.508456	13.022810
14.414559	352.560452	13.027827
14.643576	349.972131	13.032845
14.548480	344.935007	13.037863
13.904141	344.003682	13.042880
13.984585	330.131847	13.047898
14.285931	350.906073	13.052915
14.342399	342.178500	13.057933
14.707147	342.311296	13.062951
14.374298	338.469310	13.067968
14.175930	335.139690	13.072986
14.561062	327.680007	13.078003
14.794329	333.929963	13.083021
14.406327	334.015866	13.088039
14.218303	334.827987	13.093056
14.336854	332.925862	13.098074
14.145534	338.617109	13.103091
14.237599	340.673121	13.108109
14.595977	345.625569	13.113127
14.143276	347.330921	13.118144
14.445285	336.384574	13.123162
14.725446	354.151625	13.128179
14.574423	353.948181	13.133197
14.423155	338.395748	13.138215
14.379864	345.326205	13.143232
14.445404	345.852707	13.148250
14.718867	348.764056	13.153267
14.574197	350.194243	13.158285
14.665962	339.580415	13.163303
14.374863	339.566028	13.168320
14.945584	338.063691	13.173338
14.169438	340.690358	13.178355
14.298767	349.979603	13.183373
14.749592	347.691245	13.188391
14.651900	353.838111	13.193408
14.828928	350.778226	13.198426
15.085506	353.427131	13.203443
14.951773	349.036616	13.208461
14.758377	333.834711	13.213479
14.166687	341.260783	13.218496
14.551701	339.175167	13.223514
14.934985	345.685777	13.228531
15.219153	358.437900	13.233549
14.895693	347.588929	13.238567
14.762781	347.120746	13.243584
14.823289	341.229464	13.248602
14.962787	335.960167	13.253619
14.220806	344.955903	13.258637
15.094376	342.844710	13.263655
14.682130	356.528881	13.268672
14.914566	359.090032	13.273690
14.813999	351.936323	13.278707
15.067160	352.430458	13.283725
15.330601	350.130251	13.288743
14.765081	351.446092	13.293760
15.232058	345.535701	13.298778
14.925037	361.311460	13.303795
15.095159	354.298632	13.308813
15.366447	351.072601	13.313831
15.043320	351.757442	13.318848
14.809836	331.758897	13.323866
14.802101	349.554990	13.328883
14.852221	348.815326	13.333901
14.973828	341.444002	13.338919
14.993603	350.239092	13.343936
14.990824	357.911133	13.348954
15.032054	353.761606	13.353971
15.131939	356.229791	13.358989
14.839818	348.840833	13.364007
14.882366	349.118464	13.369024
14.788336	351.578972	13.374042
15.027152	346.944271	13.379059
14.776601	352.303936	13.384077
15.394232	352.447850	13.389095
15.595621	367.017893	13.394112
15.228636	353.108412	13.399130
15.235370	347.746180	13.404147
15.336219	349.999630	13.409165
15.548189	351.112372	13.414183
15.138238	354.641340	13.419200
15.175497	349.444760	13.424218
15.655521	362.390442	13.429235
15.378498	364.828953	13.434253
15.295876	348.754609	13.439271
15.203042	352.461409	13.444288
15.452278	370.652992	13.449306
15.413166	361.520590	13.454323
15.483840	367.404573	13.459341
15.554926	372.035703	13.464359
15.022849	358.688381	13.469376
15.605673	372.154523	13.474394
15.753746	365.148280	13.479411
15.498004	369.543132	13.484429
15.849076	362.786135	13.489447
15.714638	359.377132	13.494464
15.282673	355.348614	13.499482
15.194854	352.449879	13.504499
15.648578	361.704402	13.509517
15.869050	364.008653	13.514535
15.839905	362.981544	13.519552
15.578663	351.409709	13.524570
15.749863	349.303735	13.529587
15.210596	343.916067	13.534605
15.778306	348.656052	13.539623
15.837004	365.435168	13.544640
16.018710	362.652250	13.549658
16.040924	340.670009	13.554675
15.422993	342.994346	13.559693
15.438549	347.599404	13.564711
15.525676	358.245838	13.569728
15.643678	365.362619	13.574746
15.916227	367.750276	13.579763
15.730147	366.384702	13.584781
15.778474	371.798820	13.589799
15.965672	371.517470	13.594816
16.111249	362.652942	13.599834
15.859324	362.626145	13.604851
15.849089	364.660220	13.609869
15.971628	357.566441	13.614887
15.982971	361.821882	13.619904
15.916980	362.356241	13.624922
15.823792	359.063886	13.629939
15.657487	365.237216	13.634957
15.984324	355.580805	13.639975
16.147834	364.789001	13.644992
15.978011	362.584651	13.650010
16.249266	364.350848	13.655027
15.866069	374.300542	13.660045
15.901408	372.300921	13.665063
16.308253	362.089279	13.670080
16.086904	366.191612	13.675098
16.197369	355.634819	13.680115
15.933054	362.407202	13.685133
16.228703	365.898893	13.690151
16.393116	362.171974	13.695168
15.950640	366.535942	13.700186
16.316717	359.521004	13.705203
16.167356	369.046144	13.710221
16.269011	359.200740	13.715239
16.279974	369.139553	13.720256
16.389765	367.421815	13.725274
16.353155	358.636145	13.730291
16.198702	369.358067	13.735309
16.100376	359.218768	13.740327
15.964682	366.453939	13.745344
16.251623	357.823011	13.750362
16.164404	365.495580	13.755379
16.073648	362.906554	13.760397
16.201409	358.210249	13.765415
16.230723	360.771469	13.770432
16.259344	366.213898	13.775450
16.768161	366.529381	13.780467
16.690657	367.400030	13.785485
16.494691	362.473276	13.790503
16.585926	366.618455	13.795520
16.319739	372.425506	13.800538
16.430665	357.094153	13.805555
16.290370	365.396646	13.810573
16.237550	365.701749	13.815591
16.768071	375.689053	13.820608
16.627762	370.106724	13.825626
16.790749	363.025579	13.830643
16.658396	364.005749	13.835661
16.623413	359.457853	13.840679
16.504829	357.087743	13.845696
16.470631	367.664715	13.850714
16.831050	368.542917	13.855731
16.948837	386.152254	13.860749
16.735389	371.881198	13.865767
16.825262	361.841978	13.870784
16.748889	349.963663	13.875802
16.801376	350.268147	13.880819
16.582450	359.583219	13.885837
16.503156	352.262104	13.890855
17.173512	364.474446	13.895872
16.573868	369.172138	13.900890
17.244585	362.684094	13.905907
16.509986	362.464218	13.910925
16.743496	371.014612	13.915943
16.733791	371.773725	13.920960
16.805548	372.924077	13.925978
17.310382	374.786445	13.930995
16.902030	376.178798	13.936013
17.110170	377.251115	13.941031
17.215116	365.748482	13.946048
16.879418	363.743518	13.951066
17.022993	348.183038	13.956083
17.073002	370.567928	13.961101
16.929046	361.148908	13.966119
17.151430	355.992926	13.971136
16.813991	376.093507	13.976154
17.346490	366.717478	13.981171
17.252570	368.313325	13.986189
16.894451	374.977247	13.991207
17.301164	371.241003	13.996224
16.765846	372.501652	14.001242
17.015479	367.426627	14.006259
17.125634	369.691254	14.011277
16.960555	371.055196	14.016295
17.287851	383.601817	14.021312
16.927161	379.353923	14.026330
17.036674	378.835373	14.031347
17.046295	374.334174	14.036365
17.062109	379.494593	14.041383
17.142540	373.142630	14.046400
16.952017	377.448438	14.051418
17.138066	368.978373	14.056435
17.629167	382.253688	14.061453
17.475848	388.349269	14.066471
17.387058	369.625124	14.071488
17.256418	376.168426	14.076506
17.290425	369.984630	14.081523
17.625977	394.486707	14.086541
17.523460	385.023355	14.091559
17.407719	376.966328	14.096576
17.958904	389.509651	14.101594
17.572393	371.620769	14.106611
17.513759	366.429647	14.111629
17.358234	364.737440	14.116647
17.614396	366.726882	14.121664
17.390511	370.974771	14.126682
17.610926	363.979354	14.131699
17.850567	379.960336	14.136717
17.446799	368.331789	14.141735
17.399434	368.427769	14.146752
17.390142	381.847261	14.151770
17.842016	375.118744	14.156787
17.794015	380.125006	14.161805
17.935442	378.493855	14.166823
17.730813	372.697489	14.171840
17.575318	373.299429	14.176858
17.952654	375.449878	14.181875
17.879461	379.257762	14.186893
17.774008	383.585039	14.191911
17.780954	365.171024	14.196928
17.415146	363.880768	14.201946
18.162566	369.659385	14.206963
18.100380	377.564735	14.211981
17.563474	372.362874	14.216999
18.313475	372.981614	14.222016
17.742974	373.326294	14.227034
18.164298	379.111507	14.232051
17.872404	368.263920	14.237069
18.143225	378.392641	14.242087
18.183647	360.449922	14.247104
17.686689	368.460827	14.252122
17.799829	366.682611	14.257139
18.336618	373.775215	14.262157
17.851825	370.512273	14.267175
18.391524	377.563402	14.272192
17.985931	367.228954	14.277210
18.121925	375.608350	14.282227
18.266464	378.883742	14.287245
18.212991	378.352700	14.292263
18.063141	360.600543	14.297280
17.894451	367.686226	14.302298
18.755936	371.793528	14.307315
18.319428	370.419609	14.312333
18.095763	368.018525	14.317351
18.186950	354.924441	14.322368
18.285460	373.202607	14.327386
18.231814	376.442587	14.332403
18.365206	374.399298	14.337421
18.268368	381.189792	14.342439
18.620425	376.752035	14.347456
18.394622	376.913665	14.352474
18.198391	370.159832	14.357491
18.325160	372.589122	14.362509
18.121270	389.286075	14.367527
18.709085	380.371617	14.372544
18.338775	388.511129	14.377562
18.278371	391.139968	14.382579
18.278670	383.023847	14.387597
18.182212	384.342395	14.392615
18.647308	366.371417	14.397632
18.181894	381.070536	14.402650
18.465824	385.318254	14.407667
18.563071	383.006051	14.412685
18.588337	388.739329	14.417703
18.596029	387.239447	14.422720
18.776546	389.193335	14.427738
18.557192	384.377508	14.432755
18.423646	385.815433	14.437773
18.568629	383.281214	14.442791
18.612725	386.029475	14.447808
18.548634	382.975569	14.452826
18.666475	383.781093	14.457843
19.095359	391.575280	14.462861
18.776437	387.904675	14.467879
18.926578	374.198670	14.472896
18.874052	392.320500	14.477914
18.713464	389.407844	14.482931
18.523395	379.532113	14.487949
18.627415	390.216960	14.492967
19.002552	405.116571	14.497984
19.143073	407.439587	14.503002
18.939062	396.553055	14.508019
19.001330	384.574240	14.513037
18.936467	387.345777	14.518055
19.379798	378.232921	14.523072
18.978125	377.819205	14.528090
18.863276	379.961083	14.533107
19.327487	374.464503	14.538125
18.752020	379.171056	14.543143
18.948189	381.927195	14.548160
18.970653	379.137511	14.553178
19.253753	388.686843	14.558195
19.595477	386.724720	14.563213
18.731484	392.277733	14.568231
19.076608	380.731384	14.573248
19.071304	385.746778	14.578266
19.497023	396.233226	14.583283
19.223317	392.240015	14.588301
19.333005	396.726294	14.593319
19.467428	382.135993	14.598336
19.045910	372.182699	14.603354
19.043065	382.338253	14.608371
19.889262	387.495613	14.613389
19.551020	379.867683	14.618407
19.003992	362.584441	14.623424
19.478369	373.785941	14.628442
19.308523	384.251506	14.633459
19.357336	382.701043	14.638477
19.504223	391.129241	14.643495
19.595493	393.923804	14.648512
19.151837	387.148530	14.653530
19.295435	389.310127	14.658547
19.501830	398.372815	14.663565
19.729913	400.016356	14.668583
19.471590	396.295291	14.673600
19.942699	390.062366	14.678618
19.715205	391.035261	14.683635
19.670827	392.648642	14.688653
19.794262	395.110010	14.693671
18.979735	374.719069	14.698688
19.360337	399.453969	14.703706
19.579728	394.295287	14.708723
19.949753	388.172770	14.713741
19.619523	399.411203	14.718759
19.874569	388.440579	14.723776
20.113236	386.898424	14.728794
19.696654	389.544850	14.733811
19.940857	394.694960	14.738829
19.693942	401.120683	14.743847
19.954998	399.748602	14.748864
20.247262	394.395546	14.753882
19.839503	407.649891	14.758899
19.874814	403.567542	14.763917
19.736163	400.443195	14.768935
19.617705	399.956983	14.773952
19.687601	398.624131	14.778970
19.797946	397.300761	14.783987
19.834278	397.169126	14.789005
19.545406	405.744068	14.794023
19.874333	405.402783	14.799040
19.906100	400.276467	14.804058
19.961777	401.694399	14.809075
19.602030	403.899655	14.814093
20.291764	412.906030	14.819111
20.486402	415.946422	14.824128
20.144135	408.233904	14.829146
20.298278	408.143883	14.834163
20.117769	394.984780	14.839181
20.325731	393.207576	14.844199
19.699365	394.611785	14.849216
20.287384	402.422223	14.854234
20.438691	417.634391	14.859251
20.573958	406.281638	14.864269
20.225722	400.873676	14.869287
20.264242	401.076199	14.874304
20.269072	405.301109	14.879322
20.575405	410.766582	14.884339
20.149385	403.392138	14.889357
20.097881	407.483815	14.894375
19.785162	412.808998	14.899392
20.584657	406.278799	14.904410
20.253267	412.127571	14.909427
20.456114	409.666386	14.914445
20.468148	409.970858	14.919463
20.501627	415.974252	14.924480
20.298547	416.921257	14.929498
20.106129	412.596666	14.934515
20.351173	401.510832	14.939533
20.495586	417.456184	14.944551
20.924159	416.247359	14.949568
20.727262	415.101205	14.954586
20.494139	410.849220	14.959603
20.963738	415.560320	14.964621
21.095669	408.951028	14.969639
20.853100	411.605077	14.974656
20.848290	408.567182	14.979674
20.512865	413.924302	14.984691
20.924369	405.971356	14.989709
20.966041	415.066010	14.994727
20.792044	407.504010	14.999744
20.886118	412.611231	15.004762
20.602945	412.352625	15.009779
20.680422	411.482473	15.014797
20.576029	419.466993	15.019815
21.029954	431.981310	15.024832
21.103629	433.579471	15.029850
21.303448	439.313988	15.034867
21.369556	420.300598	15.039885
20.839269	413.617693	15.044903
20.966749	419.764235	15.049920
21.086873	401.881644	15.054938
20.884522	406.504866	15.059955
21.099865	409.232780	15.064973
20.993844	410.839982	15.069991
20.882900	422.722752	15.075008
21.240120	422.736806	15.080026
21.565642	437.558967	15.085043
21.064512	416.440717	15.090061
21.237568	419.408734	15.095079
21.192209	425.765217	15.100096
21.415751	419.586605	15.105114
21.356958	424.771276	15.110131
21.537616	422.594397	15.115149
21.667736	408.052079	15.120167
21.475319	406.719045	15.125184
21.256321	393.480733	15.130202
21.118686	402.022659	15.135219
21.164600	402.205097	15.140237
21.399327	419.890931	15.145255
21.583505	422.661566	15.150272
21.457072	423.568238	15.155290
21.722161	431.258562	15.160307
21.913234	424.949311	15.165325
21.316400	412.656550	15.170343
21.090354	407.519882	15.175360
21.545030	413.183155	15.180378
21.247204	416.972375	15.185395
21.526431	418.645823	15.190413
21.604654	418.854787	15.195431
21.299238	425.835555	15.200448
21.686251	418.921470	15.205466
21.634649	415.288130	15.210483
21.729874	423.443534	15.215501
21.644526	416.240094	15.220519
21.461120	424.498838	15.225536
21.960508	421.006917	15.230554
21.880913	428.410096	15.235571
21.697025	426.286819	15.240589
21.714616	422.327140	15.245607
21.690145	426.291541	15.250624
21.929417	417.765831	15.255642
21.860914	426.315939	15.260659
21.739900	427.086074	15.265677
21.738533	423.798344	15.270695
21.912679	437.643732	15.275712
22.258731	436.239481	15.280730
22.507594	447.700191	15.285747
22.400009	433.813371	15.290765
22.545704	424.080989	15.295783
22.214946	410.680193	15.300800
22.294933	417.206495	15.305818
22.284862	418.697779	15.310835
22.194646	413.953351	15.315853
22.317450	414.256355	15.320871
21.975200	409.071510	15.325888
22.418227	415.989390	15.330906
22.361125	417.150341	15.335923
22.219900	411.037992	15.340941
22.269859	415.760782	15.345959
22.256356	422.831792	15.350976
22.163011	417.280003	15.355994
22.018848	417.258517	15.361011
21.993926	412.920470	15.366029
22.169425	415.925973	15.371047
22.002845	421.140048	15.376064
22.364307	429.370762	15.381082
22.313229	434.535301	15.386099
22.202803	435.319566	15.391117
22.411804	438.745871	15.396135
22.656871	442.390613	15.401152
22.718359	430.048988	15.406170
22.426375	435.206856	15.411187
22.410321	443.098742	15.416205
22.837015	435.594675	15.421223
22.544176	442.677628	15.426240
22.847192	440.229244	15.431258
22.745373	440.280057	15.436275
22.556002	440.559085	15.441293
23.025678	438.062663	15.446311
22.833372	441.642965	15.451328
22.824983	430.139002	15.456346
22.785689	445.554431	15.461363
22.705878	443.115160	15.466381
23.110745	440.524691	15.471399
22.829237	444.207240	15.476416
22.970610	446.331323	15.481434
23.030771	434.715703	15.486451
23.000540	436.074433	15.491469
23.097970	432.114944	15.496487
22.900204	444.475127	15.501504
23.326046	431.186879	15.506522
22.974785	437.811889	15.511539
23.326103	432.086727	15.516557
23.152404	439.977910	15.521575
22.711646	440.447550	15.526592
23.087613	444.071912	15.531610
22.810521	436.996143	15.536627
23.393313	436.015758	15.541645
23.247553	434.262066	15.546663
23.260254	442.436639	15.551680
23.310889	439.386951	15.556698
22.935922	435.418964	15.561715
22.559051	433.549784	15.566733
23.126286	442.275460	15.571751
23.070461	440.665548	15.576768
23.719692	425.389173	15.581786
23.134510	435.802674	15.586803
23.314438	438.943186	15.591821
23.692281	434.321528	15.596839
23.355816	435.541754	15.601856
23.303383	435.496519	15.606874
23.273392	439.584854	15.611891
23.514102	441.027627	15.616909
23.483660	424.184577	15.621927
23.284718	438.681316	15.626944
23.663522	444.981232	15.631962
23.715706	452.960323	15.636979
23.391246	447.936791	15.641997
23.734433	453.551167	15.647015
24.131371	450.125682	15.652032
23.774711	435.012222	15.657050
23.750987	437.483886	15.662067
23.352341	434.851272	15.667085
23.665638	437.314642	15.672103
23.813405	448.055825	15.677120
24.028704	452.374203	15.682138
24.030057	448.357089	15.687155
23.721870	448.458966	15.692173
24.085966	442.435179	15.697191
23.769756	440.818474	15.702208
23.532912	438.864378	15.707226
23.656654	457.198660	15.712243
23.684363	457.191438	15.717261
23.545986	451.160679	15.722279
23.631484	447.521765	15.727296
24.225652	447.337989	15.732314
24.220371	442.674999	15.737331
24.151645	445.248340	15.742349
24.036178	454.828207	15.747367
23.779055	450.194959	15.752384
23.944409	447.379861	15.757402
23.750237	449.767616	15.762419
24.139471	456.185827	15.767437
24.405296	458.129596	15.772455
24.430899	470.467643	15.777472
24.717420	458.848320	15.782490
24.513452	452.357579	15.787507
24.175106	449.204358	15.792525
24.051463	443.884486	15.797543
24.403417	447.165465	15.802560
24.608037	458.715118	15.807578
24.518909	447.296295	15.812595
24.729368	448.668042	15.817613
24.854784	437.114841	15.822631
24.482693	433.168496	15.827648
24.444698	444.061670	15.832666
24.570574	440.148240	15.837683
24.635737	442.290499	15.842701
24.746692	436.328217	15.847719
24.914318	436.248720	15.852736
24.452022	445.112602	15.857754
24.707735	435.602914	15.862771
24.490931	432.951455	15.867789
24.570370	417.672286	15.872807
24.590839	433.643262	15.877824
24.744782	438.024835	15.882842
24.542999	431.874573	15.887859
24.397581	443.778503	15.892877
25.042462	449.623602	15.897895
25.108389	452.807111	15.902912
24.839913	449.043436	15.907930
24.860140	449.659044	15.912947
24.814070	464.712644	15.917965
25.005040	456.689874	15.922983
25.037429	454.599189	15.928000
25.138335	460.386982	15.933018
25.560501	449.320876	15.938035
25.208453	445.100022	15.943053
25.144520	434.661848	15.948071
24.979630	428.357527	15.953088
25.215808	431.804845	15.958106
25.038401	431.482436	15.963123
24.781485	437.348023	15.968141
25.264082	438.557484	15.973159
25.326690	452.874664	15.978176
25.414224	445.379220	15.983194
25.314641	429.610386	15.988211
24.734161	446.022060	15.993229
25.329880	446.809986	15.998247
25.136865	441.743900	16.003264
25.339768	449.667967	16.008282
25.604369	452.564934	16.013299
25.420048	453.868766	16.018317
25.529314	441.652232	16.023335
25.451660	452.450605	16.028352
25.510253	458.099825	16.033370
25.447851	449.523243	16.038387
25.402424	460.079929	16.043405
25.178671	450.777421	16.048423
25.560880	453.911686	16.053440
25.147098	453.506165	16.058458
25.658787	455.395876	16.063475
25.208181	452.862863	16.068493
25.362198	449.607738	16.073511
26.105047	470.149271	16.078528
26.111874	472.521513	16.083546
25.889284	459.820173	16.088563
25.728889	452.230790	16.093581
25.743315	440.688556	16.098599
25.951559	447.349527	16.103616
25.604594	458.218235	16.108634
26.004626	451.393624	16.113651
26.300156	459.861825	16.118669
25.890751	455.192328	16.123687
25.919358	454.673749	16.128704
25.629417	465.369489	16.133722
25.848464	465.834226	16.138739
26.154165	468.942538	16.143757
26.097526	466.177779	16.148775
26.304697	467.493238	16.153792
26.673301	464.236256	16.158810
26.342442	457.446548	16.163827
26.164120	455.742103	16.168845
26.283207	444.862037	16.173863
26.074690	449.820731	16.178880
25.998251	456.260955	16.183898
26.387711	458.595710	16.188915
26.408538	462.934902	16.193933
26.385791	461.095786	16.198951
26.476664	463.404451	16.203968
26.410914	468.801647	16.208986
26.126355	465.520134	16.214003
26.043763	465.858274	16.219021
26.165496	454.823163	16.224039
26.546729	465.906686	16.229056
26.370936	465.994262	16.234074
26.548316	459.037064	16.239091
26.406646	464.083179	16.244109
26.755813	468.235558	16.249127
27.050859	471.465444	16.254144
26.296323	463.959094	16.259162
26.899349	459.131964	16.264179
26.335737	472.407467	16.269197
26.517327	469.233249	16.274215
26.848717	473.192745	16.279232
26.578372	476.160383	16.284250
26.888959	461.362716	16.289267
26.583661	475.371140	16.294285
26.697109	467.849562	16.299303
27.095892	465.026518	16.304320
26.743252	474.185752	16.309338
26.635566	464.133053	16.314355
27.158764	476.191668	16.319373
27.230060	478.269864	16.324391
27.168329	466.638489	16.329408
27.330711	462.495318	16.334426
26.799481	458.523254	16.339443
26.688186	461.683866	16.344461
27.068544	473.878323	16.349479
27.174609	468.065108	16.354496
27.237149	481.662832	16.359514
27.483461	474.265726	16.364531
27.461622	478.744102	16.369549
27.393211	476.404033	16.374567
27.511889	458.423784	16.379584
27.209552	462.011754	16.384602
27.385876	457.812768	16.389619
27.361923	463.522177	16.394637
27.319724	468.051056	16.399655
27.656281	466.389516	16.404672
27.665382	472.131649	16.409690
27.506974	468.697956	16.414707
27.526697	457.694504	16.419725
27.345425	460.174922	16.424743
27.308731	464.611429	16.429760
27.400620	476.876046	16.434778
27.873672	469.147008	16.439795
27.825084	478.748031	16.444813
27.887529	477.337443	16.449831
27.761123	468.335335	16.454848
27.442122	472.288803	16.459866
27.669876	472.468175	16.464883
27.896872	476.305077	16.469901
28.015597	482.203707	16.474919
27.861005	467.285967	16.479936
27.702164	477.560533	16.484954
27.842647	473.764737	16.489971
28.013777	474.173821	16.494989
27.973330	477.979783	16.500007
28.030564	467.513259	16.505024
27.883869	476.400598	16.510042
27.892490	477.324113	16.515059
28.212179	479.433059	16.520077
27.361116	471.042372	16.525095
28.131764	466.397416	16.530112
27.768124	485.564969	16.535130
27.902961	474.436291	16.540147
28.057018	472.175189	16.545165
27.865109	477.308021	16.550183
28.414473	468.292213	16.555200
28.437211	480.154209	16.560218
28.350255	469.309363	16.565235
28.213987	468.901657	16.570253
27.888410	479.154850	16.575271
28.738917	486.252302	16.580288
28.965320	482.499928	16.585306
28.747527	480.747980	16.590323
27.960553	471.107138	16.595341
27.935780	469.252559	16.600359
28.412904	487.203663	16.605376
28.455272	500.261768	16.610394
28.871760	489.433196	16.615411
29.356730	486.344277	16.620429
28.607187	477.398161	16.625447
28.681937	470.428537	16.630464
28.760220	468.595780	16.635482
28.681804	462.290606	16.640499
28.698512	464.165870	16.645517
28.896127	474.110393	16.650535
28.857744	475.072782	16.655552
28.733738	485.029519	16.660570
29.010396	476.879795	16.665587
28.773043	472.934552	16.670605
29.015367	487.428898	16.675623
29.014539	485.204531	16.680640
28.941500	493.190515	16.685658
28.936721	487.949948	16.690675
28.946855	492.912478	16.695693
28.967381	485.010902	16.700711
28.794699	482.510350	16.705728
28.966541	484.279415	16.710746
29.152202	490.091890	16.715763
29.165343	484.545590	16.720781
29.125252	492.135141	16.725799
29.689325	486.029713	16.730816
29.416247	484.608250	16.735834
29.283571	485.575854	16.740851
29.288392	478.475109	16.745869
29.281157	486.709609	16.750887
29.316603	478.720510	16.755904
29.462881	489.663913	16.760922
28.945986	487.194862	16.765939
29.154103	485.553319	16.770957
29.300367	486.250285	16.775975
29.732698	475.633840	16.780992
29.431606	485.075375	16.786010
29.633152	486.517937	16.791027
29.631824	484.221069	16.796045
29.665098	495.775335	16.801063
29.588986	490.214529	16.806080
29.940340	501.990662	16.811098
29.779034	490.863902	16.816115
29.868031	487.723030	16.821133
29.707384	487.480059	16.826151
30.079479	485.816140	16.831168
29.869765	482.885871	16.836186
29.932069	494.388282	16.841203
29.758440	476.229473	16.846221
29.978808	491.613982	16.851239
30.037282	485.303264	16.856256
29.781869	494.359012	16.861274
29.799364	497.228191	16.866291
30.041923	505.262868	16.871309
29.850062	505.157294	16.876327
30.254260	497.082373	16.881344
30.542581	501.143252	16.886362
30.244043	499.694195	16.891379
30.316503	489.600811	16.896397
30.172029	509.453758	16.901415
30.433720	495.064446	16.906432
30.274767	496.784035	16.911450
30.377243	496.654723	16.916467
30.741794	497.024227	16.921485
30.436995	489.473089	16.926503
29.899144	473.469508	16.931520
30.174373	491.297424	16.936538
30.436889	489.814661	16.941555
30.522769	489.056801	16.946573
30.494504	495.256019	16.951591
30.613783	490.204410	16.956608
30.345818	494.822093	16.961626
30.339157	490.348645	16.966643
30.749834	491.578775	16.971661
30.783254	494.492809	16.976679
30.572594	493.882100	16.981696
30.602216	500.539346	16.986714
30.655105	498.978772	16.991731
30.783090	490.000159	16.996749
30.739889	490.537285	17.001767
30.676724	492.901493	17.006784
30.719122	493.699834	17.011802
31.040240	498.096418	17.016819
31.038178	498.125388	17.021837
31.024761	505.237441	17.026855
31.022633	497.692822	17.031872
31.282152	500.492763	17.036890
30.854035	503.046332	17.041907
31.308090	503.146291	17.046925
31.079205	505.804535	17.051943
31.409907	502.594471	17.056960
31.173349	488.920183	17.061978
31.509941	503.040119	17.066995
31.274034	485.708315	17.072013
31.206893	500.948256	17.077031
31.518971	498.167108	17.082048
31.417089	499.833631	17.087066
31.239967	498.289935	17.092083
31.653672	502.672104	17.097101
31.373868	504.208547	17.102119
31.779220	502.608873	17.107136
31.428951	499.302872	17.112154
31.348236	503.373873	17.117171
31.374353	496.276117	17.122189
31.422153	501.040290	17.127207
31.697995	508.441809	17.132224
31.554901	510.335647	17.137242
31.467734	511.898899	17.142259
31.855009	500.216527	17.147277
31.696068	510.472194	17.152295
31.616734	508.569303	17.157312
31.510243	504.041970	17.162330
31.272950	512.173451	17.167347
31.889549	501.421008	17.172365
31.669384	507.189382	17.177383
31.914476	517.653534	17.182400
32.070802	527.342596	17.187418
31.774410	521.383750	17.192435
32.261481	528.660875	17.197453
32.375278	521.517901	17.202471
32.529030	520.086781	17.207488
32.298684	510.466546	17.212506
31.862407	509.430236	17.217523
32.042752	496.552530	17.222541
32.141203	516.033162	17.227559
32.430304	514.044506	17.232576
32.605998	513.894328	17.237594
32.118281	513.629699	17.242611
32.477986	509.783985	17.247629
32.687561	515.936713	17.252647
32.355786	511.173066	17.257664
32.385268	501.414556	17.262682
32.630321	512.386774	17.267699
32.884271	504.067011	17.272717
32.233899	493.470811	17.277735
32.667701	504.328433	17.282752
32.755830	505.280594	17.287770
32.670705	507.253765	17.292787
32.617766	491.947807	17.297805
32.419000	500.937936	17.302823
32.410879	507.948185	17.307840
32.793658	496.698842	17.312858
32.441503	512.358692	17.317875
32.928692	505.277504	17.322893
32.839274	506.203662	17.327911
32.630565	499.546391	17.332928
32.751913	502.560341	17.337946
32.834781	505.472990	17.342963
32.972737	507.165286	17.347981
32.778057	507.341005	17.352999
32.809589	506.752545	17.358016
33.301468	518.118663	17.363034
33.310072	520.575838	17.368051
33.086026	515.909021	17.373069
33.459009	520.401673	17.378087
33.452185	512.400206	17.383104
33.198123	509.969122	17.388122
33.152854	512.500952	17.393139
33.445904	511.821284	17.398157
33.796932	513.988469	17.403175
33.358513	501.601557	17.408192
33.180298	511.014506	17.413210
33.786259	523.262232	17.418227
33.408960	517.925027	17.423245
33.685518	520.690763	17.428263
33.594010	520.657923	17.433280
33.702819	513.430525	17.438298
33.412380	522.103593	17.443315
33.868226	515.421740	17.448333
34.013594	525.838311	17.453351
33.674770	507.982889	17.458368
33.670244	507.160212	17.463386
33.967611	519.894619	17.468403
33.888192	520.087105	17.473421
33.922293	518.857644	17.478439
34.015092	520.531726	17.483456
34.067780	519.160522	17.488474
34.064985	523.437137	17.493491
33.900704	515.258222	17.498509
33.929077	517.778587	17.503527
34.218320	515.723640	17.508544
34.179784	525.124317	17.513562
34.154655	522.054854	17.518579
34.078341	520.744758	17.523597
34.269747	520.428039	17.528615
34.265064	521.845911	17.533632
34.452099	522.350347	17.538650
34.111458	517.547055	17.543667
34.334153	504.527055	17.548685
34.392092	517.055752	17.553703
34.226769	518.880472	17.558720
34.590691	513.456265	17.563738
34.319570	514.742059	17.568755
34.522264	511.971628	17.573773
34.396740	516.182147	17.578791
34.264924	516.707825	17.583808
34.389221	509.115116	17.588826
34.254347	521.108971	17.593843
34.466070	515.263511	17.598861
34.434129	511.046447	17.603879
34.563097	524.936806	17.608896
34.709653	522.916697	17.613914
34.739559	529.649646	17.618931
35.032659	536.792880	17.623949
35.131898	528.800138	17.628967
34.964554	536.377964	17.633984
34.990473	531.817385	17.639002
34.748687	533.515161	17.644019
34.869988	531.486360	17.649037
35.029484	531.843611	17.654055
34.863931	531.557223	17.659072
34.955914	535.721260	17.664090
35.279276	529.435554	17.669107
35.343273	528.993510	17.674125
35.053150	532.961429	17.679143
35.297526	540.800188	17.684160
35.533194	522.814281	17.689178
35.608548	527.700398	17.694195
35.137190	525.956367	17.699213
35.532546	528.735164	17.704231
35.317538	530.176317	17.709248
36.014502	523.971294	17.714266
35.717885	526.157269	17.719283
35.392774	527.533516	17.724301
35.769396	529.466355	17.729319
35.558091	534.630624	17.734336
35.362160	524.673677	17.739354
35.252669	529.995655	17.744371
35.495997	533.722735	17.749389
36.092999	520.019623	17.754407
35.605899	524.497870	17.759424
35.786792	520.591634	17.764442
35.974076	532.374400	17.769459
36.008095	532.807989	17.774477
36.333885	528.304860	17.779495
35.953333	528.395915	17.784512
35.793858	532.005835	17.789530
36.013812	529.396809	17.794547
36.191540	536.529605	17.799565
36.633567	538.445950	17.804583
36.173502	523.102371	17.809600
36.368370	515.435558	17.814618
36.179701	524.133806	17.819635
36.126468	521.614650	17.824653
36.711953	514.038492	17.829671
36.337529	515.356148	17.834688
36.225152	511.678604	17.839706
36.123689	510.148372	17.844723
36.246187	523.282377	17.849741
36.531110	535.867261	17.854759
36.486934	547.985863	17.859776
36.769736	537.200166	17.864794
36.469086	538.244416	17.869811
36.700441	536.807524	17.874829
36.869424	538.529705	17.879847
36.468082	541.666065	17.884864
36.898869	532.242672	17.889882
36.941015	529.907472	17.894899
36.987554	532.058953	17.899917
37.038145	529.959114	17.904935
36.724300	543.905809	17.909952
37.148619	533.075991	17.914970
37.149136	530.302323	17.919987
37.058651	521.584917	17.925005
36.728744	510.074158	17.930023
36.899237	526.327960	17.935040
37.112678	526.686279	17.940058
37.148511	533.980017	17.945075
37.028995	532.165427	17.950093
37.556936	540.783667	17.955111
37.276784	534.866467	17.960128
37.295867	529.208779	17.965146
37.325027	525.231496	17.970163
37.153158	530.938712	17.975181
37.451394	523.965828	17.980199
37.363997	527.053306	17.985216
37.404312	524.955067	17.990234
37.335046	525.818130	17.995251
37.051310	532.205454	18.000269
37.556483	526.850766	18.005287
36.830428	523.527531	18.010304
37.453217	532.323496	18.015322
37.620590	541.117790	18.020339
37.722743	544.425058	18.025357
38.003664	542.327224	18.030375
38.133711	539.937313	18.035392
37.973080	538.151214	18.040410
37.838199	534.953675	18.045427
37.705114	534.589652	18.050445
38.209919	536.395240	18.055463
38.396496	535.470228	18.060480
38.233215	533.630895	18.065498
38.166602	526.831575	18.070515
37.940153	524.389878	18.075533
37.682786	524.060983	18.080551
37.955225	538.285606	18.085568
38.343231	532.658837	18.090586
38.606057	538.497182	18.095603
38.200690	543.896787	18.100621
38.583826	540.303028	18.105639
38.251927	543.046741	18.110656
38.308796	538.023769	18.115674
38.287917	543.578097	18.120691
38.155542	541.790754	18.125709
38.248642	537.516347	18.130727
38.320705	535.712953	18.135744
38.333614	541.549187	18.140762
38.385377	543.740880	18.145779
38.544555	555.442833	18.150797
38.684613	553.366930	18.155815
38.825594	561.218640	18.160832
39.050338	560.593785	18.165850
38.997586	558.181842	18.170867
38.746381	558.798690	18.175885
39.073340	547.043630	18.180903
39.347747	553.482911	18.185920
38.852206	538.864336	18.190938
38.819634	549.393828	18.195955
38.539571	553.783046	18.200973
38.865673	546.524959	18.205991
39.031451	555.085988	18.211008
38.787626	558.497617	18.216026
38.719501	554.936245	18.221043
38.896845	553.851730	18.226061
39.388060	555.874023	18.231079
39.345610	569.033743	18.236096
39.831631	567.317367	18.241114
39.476371	545.494623	18.246131
39.509483	548.598055	18.251149
39.704912	550.306652	18.256167
39.936184	541.551763	18.261184
39.729925	547.747157	18.266202
39.226001	540.902313	18.271219
39.332502	547.929444	18.276237
39.484869	532.796605	18.281255
40.123239	552.830661	18.286272
40.071510	549.014284	18.291290
40.281080	538.710184	18.296307
39.625214	540.765908	18.301325
39.264475	536.966089	18.306343
39.925990	549.883653	18.311360
39.879019	556.887348	18.316378
40.204156	551.775269	18.321395
40.351542	563.302346	18.326413
40.177038	552.010351	18.331431
39.988786	549.591104	18.336448
39.935619	552.932023	18.341466
40.402353	556.826288	18.346483
40.026827	556.910248	18.351501
40.775366	558.046756	18.356519
40.556442	548.468900	18.361536
40.318940	548.648131	18.366554
40.368497	551.401879	18.371571
40.438797	548.844552	18.376589
40.319223	564.051687	18.381607
40.464539	557.456034	18.386624
40.550684	559.601353	18.391642
40.578506	558.088855	18.396659
39.946991	563.457408	18.401677
40.312386	554.252458	18.406695
40.567429	557.681085	18.411712
40.569334	558.552003	18.416730
40.699719	556.130481	18.421747
40.791024	567.435928	18.426765
40.844572	561.779175	18.431783
41.116969	572.456851	18.436800
40.949630	572.735607	18.441818
41.094203	570.624286	18.446835
41.367223	574.062740	18.451853
41.369529	566.640472	18.456871
41.106456	555.665209	18.461888
41.169144	560.414457	18.466906
41.324878	550.749867	18.471923
40.990130	553.617096	18.476941
41.178832	558.933680	18.481959
41.767531	569.789316	18.486976
41.454318	558.484201	18.491994
41.161992	551.215105	18.497011
41.325438	567.870814	18.502029
41.621457	570.052882	18.507047
41.746501	564.186189	18.512064
41.770917	573.766432	18.517082
41.631520	566.325202	18.522099
41.353119	575.517109	18.527117
41.663267	564.853365	18.532135
41.796147	565.577664	18.537152
41.805327	558.321580	18.542170
42.024665	561.878838	18.547187
41.861000	563.371958	18.552205
42.136689	570.893443	18.557223
42.095443	561.950610	18.562240
42.035456	565.014893	18.567258
42.163224	566.759272	18.572275
41.793648	570.777438	18.577293
41.836693	568.145459	18.582311
42.087529	565.007777	18.587328
41.964386	558.879937	18.592346
42.119599	560.534839	18.597363
42.032292	567.721536	18.602381
42.057313	559.178624	18.607399
42.066614	558.315924	18.612416
41.753766	565.118031	18.617434
42.207537	577.178059	18.622451
42.543851	584.614375	18.627469
42.610732	578.835625	18.632487
42.637272	580.100324	18.637504
42.445908	588.824268	18.642522
42.748545	577.988123	18.647539
42.594966	591.203031	18.652557
43.176035	581.790925	18.657575
43.188328	581.151811	18.662592
42.925867	585.004986	18.667610
43.020678	577.098114	18.672627
43.085869	584.119069	18.677645
42.951939	572.164362	18.682663
42.776470	560.443339	18.687680
42.676940	574.949959	18.692698
43.041595	571.513699	18.697715
43.112334	568.082177	18.702733
43.170903	567.155004	18.707751
43.220861	570.606097	18.712768
42.702200	578.446914	18.717786
43.299702	566.782258	18.722803
43.319706	569.130371	18.727821
43.443253	565.832634	18.732839
43.659663	565.616158	18.737856
43.192692	573.041842	18.742874
43.706001	565.789313	18.747891
43.492871	580.152684	18.752909
43.617276	579.849551	18.757927
44.066879	576.920752	18.762944
43.539833	579.906284	18.767962
43.743417	573.875887	18.772979
43.883531	571.907265	18.777997
43.982059	573.908652	18.783015
44.090430	568.852407	18.788032
43.831271	569.094968	18.793050
44.378594	565.743873	18.798067
44.152980	563.545028	18.803085
44.178234	562.458946	18.808103
44.138246	562.560090	18.813120
44.069421	559.323862	18.818138
44.004920	553.433037	18.823155
44.211997	566.105800	18.828173
44.228062	575.475913	18.833191
44.589001	571.131396	18.838208
44.488635	573.390958	18.843226
44.583771	563.123594	18.848243
44.395438	553.793427	18.853261
44.166196	559.279220	18.858279
44.604814	562.269028	18.863296
44.732590	572.991312	18.868314
44.641409	570.367608	18.873331
44.816798	568.923649	18.878349
44.708116	568.978686	18.883367
45.156025	572.654988	18.888384
44.677786	573.281939	18.893402
44.846709	569.570053	18.898419
44.812670	567.619079	18.903437
44.864297	572.013461	18.908455
44.649851	564.602851	18.913472
45.075269	570.018277	18.918490
45.104241	570.487366	18.923507
44.886435	570.010305	18.928525
44.686038	572.392734	18.933543
44.984408	567.313220	18.938560
44.939364	571.315570	18.943578
45.064019	573.297110	18.948595
45.076302	570.322796	18.953613
45.180755	573.746471	18.958631
45.409656	587.299442	18.963648
45.304781	597.079701	18.968666
45.985627	581.006192	18.973683
45.796713	584.611239	18.978701
45.563440	577.175154	18.983719
45.892933	567.224736	18.988736
45.641898	573.263014	18.993754
45.653883	573.668478	18.998771
46.173799	565.203139	19.003789
45.683811	565.775117	19.008807
45.761995	569.076654	19.013824
45.975747	571.397758	19.018842
45.933823	581.149274	19.023859
46.044270	582.861639	19.028877
46.047564	585.449032	19.033895
46.322230	578.331479	19.038912
46.131228	584.183696	19.043930
46.394311	582.893334	19.048947
46.462445	582.532693	19.053965
46.112634	585.537966	19.058983
46.085885	577.997145	19.064000
46.138101	577.361283	19.069018
46.129169	583.851001	19.074035
46.074777	568.658807	19.079053
46.043902	579.005024	19.084071
46.372543	583.817008	19.089088
46.826450	585.778844	19.094106
46.850654	591.502887	19.099123
46.354854	585.499328	19.104141
46.341223	597.319730	19.109159
46.806064	592.400475	19.114176
47.091800	602.962489	19.119194
46.976163	596.158151	19.124211
47.189334	592.581377	19.129229
47.151277	593.098771	19.134247
47.349309	589.401282	19.139264
47.086257	588.858685	19.144282
47.195301	585.885081	19.149299
47.412126	593.624016	19.154317
47.363207	589.535804	19.159335
47.084812	579.648467	19.164352
47.303993	588.882826	19.169370
47.735662	586.089356	19.174387
47.534100	583.302962	19.179405
47.004579	580.087966	19.184423
47.467072	579.224131	19.189440
47.765712	583.889313	19.194458
47.738546	577.610830	19.199475
47.395116	579.195053	19.204493
47.455003	590.404425	19.209511
48.065036	575.541105	19.214528
47.582761	587.437622	19.219546
47.566048	583.801971	19.224563
47.498821	575.655251	19.229581
47.209209	580.279482	19.234599
47.918477	583.372317	19.239616
47.973227	595.223095	19.244634
48.201516	598.018447	19.249651
48.384061	594.042514	19.254669
48.252563	591.557623	19.259687
48.266779	581.293379	19.264704
47.918000	580.303400	19.269722
47.717568	588.741589	19.274739
48.345715	588.388428	19.279757
48.085362	596.574029	19.284775
48.412655	592.313637	19.289792
48.485808	601.182590	19.294810
48.290659	587.495466	19.299827
48.692767	585.599656	19.304845
48.273192	598.183824	19.309863
48.807410	584.673466	19.314880
48.807057	588.990742	19.319898
48.567006	594.462450	19.324915
48.435025	592.517256	19.329933
49.190103	602.043712	19.334951
48.940397	603.919446	19.339968
49.006187	605.036030	19.344986
48.955004	602.049502	19.350003
49.307143	606.330835	19.355021
49.278981	597.976059	19.360039
49.168443	586.109215	19.365056
49.462423	593.034594	19.370074
49.059514	594.331445	19.375091
49.543580	596.572598	19.380109
49.365768	604.937848	19.385127
49.332415	609.105638	19.390144
49.715074	607.793501	19.395162
49.293269	609.632917	19.400179
49.727530	608.726140	19.405197
49.984100	606.556353	19.410215
49.748571	594.418641	19.415232
49.864609	596.297388	19.420250
49.577062	593.574871	19.425267
49.580423	595.600544	19.430285
49.809636	597.837197	19.435303
49.713540	594.977579	19.440320
49.910984	607.446752	19.445338
49.748416	601.807856	19.450355
50.032323	595.913262	19.455373
49.716695	603.539450	19.460391
49.844499	607.789441	19.465408
50.382125	602.887252	19.470426
49.909940	616.000311	19.475443
50.548267	610.498639	19.480461
50.655055	626.598358	19.485479
50.260586	604.159973	19.490496
50.741116	601.917449	19.495514
50.782957	612.615269	19.500531
51.079735	593.824541	19.505549
50.561774	598.941904	19.510567
50.505397	594.782271	19.515584
50.413139	588.741127	19.520602
50.519204	603.932101	19.525619
51.042547	597.842444	19.530637
51.082695	606.359945	19.535655
51.236026	609.438359	19.540672
51.143418	600.885340	19.545690
50.948740	597.170101	19.550707
51.618559	591.414232	19.555725
51.028755	583.938984	19.560743
51.071516	578.025139	19.565760
51.279041	579.324773	19.570778
51.130931	592.936447	19.575795
51.418569	594.567579	19.580813
51.474366	607.753057	19.585831
51.156917	605.101463	19.590848
51.496695	605.424336	19.595866
51.430116	607.754379	19.600883
51.765320	608.876352	19.605901
51.461503	623.061381	19.610919
51.517384	609.745395	19.615936
52.024944	597.763375	19.620954
51.297386	600.978937	19.625971
51.744461	604.854184	19.630989
51.944110	604.996910	19.636007
51.787925	602.430657	19.641024
51.860935	608.162885	19.646042
51.617442	602.956294	19.651059
51.963269	603.385519	19.656077
51.670401	608.515173	19.661095
51.673272	606.599473	19.666112
52.342106	608.171256	19.671130
51.947227	617.160422	19.676147
52.087741	609.694527	19.681165
52.187489	615.255343	19.686183
52.257400	611.773451	19.691200
52.663104	613.405136	19.696218
52.117121	618.255478	19.701235
52.384670	613.398491	19.706253
52.685725	628.019505	19.711271
52.944670	615.325126	19.716288
53.583453	618.350050	19.721306
52.767740	616.113689	19.726323
52.670748	603.269617	19.731341
52.790525	609.663570	19.736359
52.998009	621.752508	19.741376
53.492263	620.334635	19.746394
53.241760	618.654035	19.751411
53.230500	604.752081	19.756429
53.078323	599.733238	19.761447
53.361727	601.276670	19.766464
53.471476	606.318394	19.771482
53.245895	611.525933	19.776499
53.195479	612.783682	19.781517
53.295628	616.902287	19.786535
53.329855	611.573562	19.791552
53.632173	615.534463	19.796570
53.747229	620.881466	19.801587
53.930253	619.168081	19.806605
53.790410	620.950975	19.811623
53.465131	619.395622	19.816640
53.748743	608.534018	19.821658
53.242311	620.336492	19.826675
53.838387	617.365947	19.831693
53.983781	615.128265	19.836711
53.785552	621.720051	19.841728
54.046522	629.597290	19.846746
54.127525	643.536236	19.851763
54.381468	634.427489	19.856781
54.555505	629.067524	19.861799
54.651613	637.629975	19.866816
54.285276	620.782230	19.871834
54.401263	636.470286	19.876851
54.224689	629.078998	19.881869
54.374808	635.802738	19.886887
54.402897	641.680822	19.891904
54.836857	627.056304	19.896922
54.631345	631.298238	19.901939
54.672040	623.952017	19.906957
54.648542	633.669135	19.911975
54.472295	630.547445	19.916992
54.811557	622.280613	19.922010
54.717834	631.368059	19.927027
54.649873	630.892912	19.932045
55.029079	634.365337	19.937063
54.860643	656.724645	19.942080
55.234424	650.068141	19.947098
55.614232	649.554835	19.952115
55.825338	648.411411	19.957133
55.680860	630.774903	19.962151
55.110647	618.989073	19.967168
55.281803	617.463721	19.972186
55.083834	639.802361	19.977203
55.048441	632.206060	19.982221
55.308672	632.361444	19.987239
55.524233	643.287846	19.992256
55.762563	631.584397	19.997274
55.772344	635.543513	20.002291
55.821745	645.037857	20.007309
56.047803	636.469918	20.012327
55.912672	635.033276	20.017344
55.866691	635.555060	20.022362
55.654130	640.407143	20.027379
56.159273	654.043384	20.032397
56.780903	657.143566	20.037415
56.347664	643.499779	20.042432
56.162808	634.257386	20.047450
56.186388	632.240632	20.052467
56.444053	646.950465	20.057485
56.704487	643.918568	20.062503
56.816133	646.668976	20.067520
56.821262	627.604895	20.072538
56.617749	630.628422	20.077555
56.569699	621.585635	20.082573
56.466145	632.994044	20.087591
56.537006	646.880925	20.092608
56.990941	636.844822	20.097626
56.453286	646.638844	20.102643
56.512063	644.017027	20.107661
57.320018	637.980870	20.112679
57.139666	640.066708	20.117696
57.353934	641.595663	20.122714
57.328877	641.158015	20.127731
57.236333	639.323436	20.132749
57.409488	643.010974	20.137767
57.138454	650.055903	20.142784
57.665224	643.997253	20.147802
57.152302	644.140474	20.152819
57.205174	643.053243	20.157837
57.846684	649.214505	20.162855
57.644495	665.217204	20.167872
57.928373	661.970222	20.172890
58.072722	661.616647	20.177907
57.889381	650.411168	20.182925
57.862008	631.484683	20.187943
57.639820	650.447363	20.192960
57.896114	655.485219	20.197978
58.369703	663.307281	20.202995
58.154668	658.115177	20.208013
58.520343	654.195921	20.213031
58.336015	649.030596	20.218048
58.532540	651.367016	20.223066
58.549301	648.215272	20.228083
58.600235	641.372359	20.233101
58.171458	637.636757	20.238119
58.179662	647.105959	20.243136
58.771447	644.824019	20.248154
58.684008	649.047575	20.253171
58.459923	658.101685	20.258189
58.716542	652.643651	20.263207
58.734947	645.562813	20.268224
58.633096	652.707630	20.273242
58.451036	654.140507	20.278259
58.537639	654.313457	20.283277
58.873255	656.991127	20.288295
59.193222	655.429980	20.293312
58.839840	661.465290	20.298330
59.333334	664.591734	20.303347
59.004771	667.445396	20.308365
59.628518	657.979269	20.313383
59.446418	670.621186	20.318400
59.474873	663.993196	20.323418
59.904573	657.482612	20.328435
59.436131	661.352095	20.333453
59.721391	655.775996	20.338471
59.629355	662.127209	20.343488
60.186325	657.338754	20.348506
60.085729	660.472491	20.353523
59.543111	658.979373	20.358541
60.050066	649.531435	20.363559
59.896061	663.358669	20.368576
60.167614	666.144141	20.373594
60.008422	661.015923	20.378611
59.997965	662.204340	20.383629
60.008994	653.606758	20.388647
59.814180	663.846010	20.393664
60.169041	655.011864	20.398682
60.144359	659.389748	20.403699
60.138858	677.428815	20.408717
60.573745	674.246679	20.413735
60.772687	691.449226	20.418752
60.875867	674.313741	20.423770
60.826317	682.826311	20.428787
60.840319	679.198480	20.433805
61.144288	670.889785	20.438823
61.122322	678.826877	20.443840
60.922631	673.342055	20.448858
61.080470	668.704099	20.453875
61.222129	671.377257	20.458893
61.115176	663.889910	20.463911
61.062178	670.948235	20.468928
61.013953	675.954616	20.473946
61.175510	659.598981	20.478963
61.041514	670.229541	20.483981
61.371917	673.280398	20.488999
61.234320	665.207706	20.494016
61.445749	671.565321	20.499034
61.281443	668.741556	20.504051
61.786676	687.796142	20.509069
61.810947	684.182490	20.514087
61.923735	693.218882	20.519104
62.161884	684.033676	20.524122
62.152858	684.073197	20.529139
62.163098	688.398315	20.534157
62.117235	683.113595	20.539175
62.280413	678.717794	20.544192
62.181918	685.568621	20.549210
62.127030	680.351577	20.554227
62.169519	682.478462	20.559245
61.983508	681.743991	20.564263
61.935458	676.980304	20.569280
62.239956	674.039368	20.574298
62.734145	671.939871	20.579315
62.437900	681.222971	20.584333
62.512295	678.197944	20.589351
62.512612	684.386468	20.594368
62.717665	690.442136	20.599386
62.908575	696.307510	20.604403
63.151186	695.541017	20.609421
63.183256	693.245233	20.614439
63.289041	695.734637	20.619456
63.185201	693.365342	20.624474
63.614978	682.648188	20.629491
63.066069	672.310626	20.634509
63.486948	671.680475	20.639527
63.038042	666.862440	20.644544
63.044299	679.582331	20.649562
63.826681	682.783718	20.654579
63.340702	690.023068	20.659597
63.675020	684.395143	20.664615
63.577116	684.710425	20.669632
63.456274	690.867324	20.674650
63.912281	681.856476	20.679667
63.529701	689.537305	20.684685
63.644070	676.571911	20.689703
63.517768	682.089051	20.694720
63.781512	685.087174	20.699738
64.038168	688.774343	20.704755
64.428002	704.637568	20.709773
64.878116	702.065263	20.714791
64.449591	688.805702	20.719808
64.239515	685.458902	20.724826
64.483534	686.588767	20.729843
64.661612	697.142354	20.734861
64.691646	689.497973	20.739879
64.373859	684.697387	20.744896
64.943240	693.435480	20.749914
64.878380	691.246302	20.754931
65.018846	690.959602	20.759949
64.888680	685.574401	20.764967
65.318024	693.072016	20.769984
64.858450	686.889218	20.775002
65.267164	688.760276	20.780019
64.860139	694.800793	20.785037
65.193081	688.074896	20.790055
64.683157	681.754777	20.795072
64.793470	689.320996	20.800090
65.235730	691.966289	20.805107
65.490074	706.490503	20.810125
65.966933	709.521720	20.815143
65.612190	698.986659	20.820160
65.837324	712.628674	20.825178
65.966253	689.386032	20.830195
65.663410	695.157873	20.835213
65.891214	690.827743	20.840231
65.548806	703.365259	20.845248
65.758923	709.574774	20.850266
66.107352	695.427405	20.855283
66.076126	700.689914	20.860301
65.640384	702.073932	20.865319
66.100159	697.953829	20.870336
66.041214	703.201721	20.875354
66.582006	708.324681	20.880371
66.433186	722.476191	20.885389
66.589752	720.820562	20.890407
66.658783	719.964333	20.895424
66.953787	717.185810	20.900442
67.163053	712.896430	20.905459
66.967249	723.602915	20.910477
67.057992	711.651001	20.915495
67.009814	701.573121	20.920512
66.911294	702.260872	20.925530
67.440290	703.576735	20.930547
67.036304	713.163795	20.935565
66.958519	705.779183	20.940583
67.186672	713.813045	20.945600
67.134486	705.758593	20.950618
67.343973	700.812795	20.955635
67.112515	708.965549	20.960653
67.160196	719.978095	20.965671
67.608657	708.948756	20.970688
67.266213	705.496334	20.975706
67.551606	711.021965	20.980723
67.649700	722.048753	20.985741
67.940156	723.016761	20.990759
68.157788	723.835165	20.995776
67.800763	733.484350	21.000794
68.071407	730.188926	21.005811
68.053847	726.742719	21.010829
68.160019	724.397525	21.015847
68.591982	725.813701	21.020864
68.405126	725.259235	21.025882
68.242124	725.382688	21.030899
68.265876	727.518807	21.035917
68.379484	715.654846	21.040935
68.817529	716.041314	21.045952
68.361663	719.981432	21.050970
68.608261	719.817058	21.055987
68.553610	714.120299	21.061005
68.476075	726.146392	21.066023
68.888312	737.685995	21.071040
68.738783	740.622244	21.076058
69.225281	740.234332	21.081075
69.346899	733.973652	21.086093
69.323326	739.556863	21.091111
69.157984	737.506397	21.096128
69.045234	738.177431	21.101146
69.701795	731.868177	21.106163
69.604411	725.357584	21.111181
69.752726	735.070098	21.116199
69.648947	728.289109	21.121216
69.368959	735.654192	21.126234
69.888434	726.907986	21.131251
69.981611	733.211454	21.136269
69.626245	728.833260	21.141287
70.001676	734.559469	21.146304
70.016029	737.082049	21.151322
70.422635	745.974895	21.156339
70.288221	749.079200	21.161357
70.462484	752.286920	21.166375
70.747987	743.899017	21.171392
70.387516	741.377173	21.176410
70.685611	738.636033	21.181427
70.828713	737.582084	21.186445
70.565724	742.631388	21.191463
70.800120	737.331419	21.196480
70.421178	750.556289	21.201498
70.679721	739.569123	21.206515
70.746396	745.567462	21.211533
70.759899	747.862965	21.216551
70.729912	739.511561	21.221568
70.711528	740.496096	21.226586
71.127447	750.249004	21.231603
71.289334	750.375521	21.236621
71.075071	757.099238	21.241639
71.293360	742.479801	21.246656
71.397266	752.805136	21.251674
71.701903	755.825306	21.256691
71.493930	754.677698	21.261709
71.491095	748.329095	21.266727
71.653335	745.397673	21.271744
71.321538	746.756044	21.276762
71.459376	757.729331	21.281779
71.952846	769.316267	21.286797
72.220995	769.950089	21.291815
72.639272	762.573423	21.296832
72.593373	771.271655	21.301850
72.676819	756.149353	21.306867
72.244034	741.741735	21.311885
72.122180	735.780885	21.316903
72.786359	748.511997	21.321920
72.626359	745.621279	21.326938
72.198064	737.436028	21.331955
72.572956	746.390615	21.336973
72.700135	758.558421	21.341991
72.927420	753.783402	21.347008
72.594653	753.867017	21.352026
72.901066	760.187786	21.357043
73.006494	764.472857	21.362061
72.596227	761.337087	21.367079
72.744390	747.593230	21.372096
73.043539	765.875281	21.377114
73.394911	776.698573	21.382131
73.578505	772.167030	21.387149
73.552535	775.049333	21.392167
73.979994	763.874912	21.397184
73.902705	773.262822	21.402202
73.929408	776.136925	21.407219
74.255752	776.856358	21.412237
73.468715	761.844333	21.417255
73.634670	763.260904	21.422272
73.934240	770.425318	21.427290
74.298521	767.424568	21.432307
74.027519	770.291374	21.437325
73.920425	772.492050	21.442343
74.409558	759.578697	21.447360
74.217672	766.289467	21.452378
73.693544	767.990199	21.457395
74.219893	775.920859	21.462413
74.300838	787.638305	21.467431
74.655860	783.029577	21.472448
74.593972	788.593524	21.477466
74.685929	778.714682	21.482483
74.808980	779.229087	21.487501
74.866918	787.289484	21.492519
74.892939	776.755052	21.497536
75.227703	791.897959	21.502554
75.209941	798.275526	21.507571
75.515234	791.856844	21.512589
75.667587	802.496549	21.517607
75.752270	789.182254	21.522624
75.850630	779.987205	21.527642
75.461333	776.863946	21.532659
75.578701	775.470028	21.537677
75.606803	794.816761	21.542695
75.890713	784.706064	21.547712
75.985872	795.402005	21.552730
76.165039	788.595873	21.557747
76.468631	784.941868	21.562765
76.214290	796.231852	21.567783
76.600612	781.914416	21.572800
76.225342	798.906677	21.577818
76.205139	791.752899	21.582835
76.213081	789.542907	21.587853
76.143675	797.080351	21.592871
76.217119	789.971951	21.597888
76.171060	791.068093	21.602906
76.030502	795.318889	21.607923
76.225297	799.009402	21.612941
76.646520	811.235602	21.617959
76.975741	804.712207	21.622976
76.755861	805.743897	21.627994
76.942204	806.639758	21.633011
76.961618	809.319347	21.638029
77.274341	819.520694	21.643047
77.752335	813.059337	21.648064
77.266597	812.043331	21.653082
77.611839	821.867241	21.658099
77.705283	813.941541	21.663117
77.535135	812.283124	21.668135
77.985691	812.311051	21.673152
77.678372	810.724482	21.678170
77.977845	816.383650	21.683187
78.426976	814.553078	21.688205
77.706139	812.484951	21.693223
77.920496	803.388592	21.698240
78.264611	815.039836	21.703258
78.310541	825.279568	21.708275
78.522025	820.216665	21.713293
78.134650	815.594130	21.718311
78.576178	814.197076	21.723328
78.297142	816.421372	21.728346
78.295846	824.550967	21.733363
78.474666	816.517302	21.738381
78.371594	824.154670	21.743399
78.771249	822.789380	21.748416
79.087835	835.334838	21.753434
79.103714	827.099325	21.758451
79.372812	819.215700	21.763469
79.518946	826.883697	21.768487
79.673156	827.819275	21.773504
79.610601	832.786908	21.778522
79.537863	831.141724	21.783539
79.591156	810.170200	21.788557
79.605820	826.846164	21.793575
79.722430	824.619249	21.798592
79.759430	816.105904	21.803610
79.697524	824.058747	21.808627
79.585569	818.629646	21.813645
79.871839	823.293664	21.818663
80.135960	813.378530	21.823680
79.892837	821.492127	21.828698
79.766382	826.223560	21.833715
80.132207	828.934422	21.838733
79.829483	836.135833	21.843751
80.247823	828.238436	21.848768
80.490779	840.312536	21.853786
80.077925	843.602216	21.858803
80.630102	835.024431	21.863821
80.832772	848.452304	21.868839
81.193933	858.138059	21.873856
81.550422	848.479918	21.878874
80.952344	843.669280	21.883891
81.667024	835.321808	21.888909
81.361774	833.012254	21.893927
81.278355	823.823394	21.898944
81.284779	835.997431	21.903962
81.600606	845.144297	21.908979
82.084008	844.586456	21.913997
82.138084	833.826721	21.919015
81.654799	827.025887	21.924032
81.887201	826.380896	21.929050
81.553902	823.217352	21.934067
81.872438	824.162059	21.939085
81.936598	838.195299	21.944103
81.994317	841.130854	21.949120
82.434973	839.140656	21.954138
81.941100	841.095455	21.959155
82.697158	842.707328	21.964173
82.904009	840.497918	21.969191
82.461085	844.824203	21.974208
82.424800	833.434769	21.979226
82.501631	840.539219	21.984243
82.584441	831.191934	21.989261
82.673435	830.244231	21.994279
82.594721	834.125654	21.999296
82.832430	831.434926	22.004314
82.608101	830.431867	22.009331
83.063927	842.210900	22.014349
83.216532	848.502001	22.019367
83.388847	842.138718	22.024384
83.560334	837.003143	22.029402
83.432328	852.754627	22.034419
83.684441	845.665724	22.039437
83.719660	850.138467	22.044455
83.665951	844.476232	22.049472
84.255125	837.719853	22.054490
83.838664	845.424958	22.059507
83.986827	828.698874	22.064525
83.937741	850.190957	22.069543
84.124684	846.476208	22.074560
84.117745	834.845523	22.079578
83.809380	835.332427	22.084595
84.067459	852.926704	22.089613
84.444515	857.813276	22.094631
84.422801	853.035973	22.099648
84.736044	856.439820	22.104666
84.648862	859.271709	22.109683
84.838478	856.206622	22.114701
84.781272	845.760844	22.119719
84.891303	849.631819	22.124736
85.162636	837.724283	22.129754
85.100627	842.666588	22.134771
85.417078	856.143022	22.139789
85.392706	863.534631	22.144807
85.576285	872.329725	22.149824
85.990423	861.084735	22.154842
85.817865	866.157864	22.159859
85.844426	858.185754	22.164877
85.999424	842.566254	22.169895
85.744007	854.058410	22.174912
86.160973	856.212217	22.179930
86.190186	857.066276	22.184947
86.021277	852.274021	22.189965
86.130037	851.408445	22.194983
85.881608	867.551067	22.200000
85.903889	853.577423	22.205018
85.769249	864.179799	22.210035
86.083915	866.882854	22.215053
86.265504	873.664902	22.220071
86.578691	870.978195	22.225088
86.951327	870.797353	22.230106
86.888918	877.393333	22.235123
86.897301	868.736099	22.240141
86.948812	874.455983	22.245159
87.229859	877.167429	22.250176
87.506381	879.724949	22.255194
87.640283	891.740326	22.260211
87.810610	880.154594	22.265229
87.839588	870.560055	22.270247
87.288335	869.055640	22.275264
87.600231	874.520394	22.280282
87.642870	885.350796	22.285299
88.127081	886.418032	22.290317
88.292538	880.503917	22.295335
88.060236	879.375866	22.300352
88.418483	869.436579	22.305370
88.292863	879.766167	22.310387
88.496341	878.961580	22.315405
88.488117	872.468607	22.320423
88.388053	867.873909	22.325440
88.740661	870.283885	22.330458
88.622988	877.352363	22.335475
88.730591	873.451149	22.340493
88.666198	867.314054	22.345511
88.688320	871.003065	22.350528
88.393075	861.294912	22.355546
88.409276	868.689673	22.360563
88.679932	879.127974	22.365581
88.877673	883.373455	22.370599
88.761699	890.255485	22.375616
89.205441	876.553869	22.380634
89.428015	879.952902	22.385651
89.697253	882.738770	22.390669
89.969004	888.635803	22.395687
89.861386	894.219526	22.400704
90.157055	890.822347	22.405722
89.916011	887.903199	22.410739
90.229332	885.816059	22.415757
90.544381	889.907582	22.420775
90.239635	892.558760	22.425792
90.535237	887.369133	22.430810
90.335370	887.526728	22.435827
90.512608	888.887906	22.440845
90.798772	885.659462	22.445863
90.896426	884.956555	22.450880
90.850038	883.704887	22.455898
90.708859	894.103176	22.460915
90.843268	884.555329	22.465933
91.147821	883.731849	22.470951
90.837989	874.284730	22.475968
91.031147	880.206619	22.480986
91.071014	889.945572	22.486003
91.191887	899.545689	22.491021
91.449901	893.951667	22.496039
91.207618	896.290169	22.501056
91.617385	895.093709	22.506074
91.745860	896.771741	22.511091
91.716749	897.152054	22.516109
92.157718	896.932171	22.521127
92.261118	897.159312	22.526144
92.385085	898.860136	22.531162
92.584929	896.980007	22.536179
92.068720	889.811896	22.541197
92.328577	898.519390	22.546215
92.852085	911.158916	22.551232
93.110582	908.884654	22.556250
93.026686	909.418661	22.561267
93.183999	896.033017	22.566285
92.889688	886.798065	22.571303
92.769720	893.740677	22.576320
92.965714	896.777787	22.581338
93.121479	899.120587	22.586355
93.087604	900.893322	22.591373
93.023483	903.630112	22.596391
93.075887	910.350237	22.601408
93.154397	902.543585	22.606426
93.077342	912.307065	22.611443
93.603593	928.243926	22.616461
93.958312	916.389626	22.621479
94.012401	919.953752	22.626496
94.239470	915.872986	22.631514
93.853095	920.749051	22.636531
93.550100	926.953327	22.641549
94.445657	928.016481	22.646567
94.461209	937.566746	22.651584
94.654036	932.595075	22.656602
95.043863	939.174317	22.661619
94.855136	942.097767	22.666637
95.202422	927.767356	22.671655
94.627648	924.231143	22.676672
94.991426	919.311754	22.681690
95.103119	937.856696	22.686707
95.181309	931.549059	22.691725
95.178333	934.260555	22.696743
95.268956	941.627981	22.701760
95.340673	929.423266	22.706778
95.724732	944.542852	22.711795
95.415724	941.782596	22.716813
95.537745	935.818421	22.721831
95.321970	942.088017	22.726848
95.763852	926.354351	22.731866
96.085435	934.099218	22.736883
95.984599	941.316575	22.741901
96.213145	954.841485	22.746919
96.384557	949.664865	22.751936
96.566955	949.280115	22.756954
96.762212	954.226577	22.761971
96.614071	948.563232	22.766989
96.741849	940.079874	22.772007
96.628864	950.609504	22.777024
96.929381	935.607883	22.782042
96.654428	946.102768	22.787059
96.391774	945.061488	22.792077
96.792977	944.955091	22.797095
96.989619	959.551614	22.802112
97.218360	958.556901	22.807130
97.629980	957.104533	22.812147
97.404106	962.154433	22.817165
97.779700	964.450393	22.822183
97.685650	970.940883	22.827200
97.955207	953.409999	22.832218
97.984947	953.642298	22.837235
97.862585	961.513099	22.842253
98.026218	969.326754	22.847271
98.459109	979.724076	22.852288
98.551342	976.380645	22.857306
98.903193	974.562047	22.862323
98.582019	981.775857	22.867341
98.705915	975.278056	22.872359
98.830811	974.914881	22.877376
98.611232	973.582875	22.882394
98.815397	970.139969	22.887411
98.648358	964.795136	22.892429
98.983608	967.056353	22.897447
98.939021	967.552684	22.902464
99.266826	977.638168	22.907482
99.754753	987.174873	22.912499
99.564651	987.485581	22.917517
99.934386	982.233893	22.922535
99.503242	991.617052	22.927552
100.081090	985.550335	22.932570
100.126172	975.656590	22.937587
100.007559	979.452740	22.942605
99.842779	985.004367	22.947623
100.065113	974.562327	22.952640
99.733706	984.466432	22.957658
100.677374	985.509476	22.962675
100.273544	1001.073666	22.967693
100.594294	1000.007822	22.972711
100.557496	1004.838951	22.977728
100.292306	1000.292017	22.982746
100.566751	989.482098	22.987763
100.784497	1000.850189	22.992781
101.427851	1004.461441	22.997799
101.650725	1003.862108	23.002816
101.730592	990.778781	23.007834
101.479117	987.065990	23.012851
101.182757	984.688760	23.017869
101.686521	994.251405	23.022887
101.993350	1004.542139	23.027904
101.694282	993.875157	23.032922
102.010809	997.190159	23.037939
102.354790	1001.485484	23.042957
102.541724	992.254443	23.047975
102.240977	990.938229	23.052992
102.254872	997.380366	23.058010
102.321587	997.111455	23.063027
102.155120	990.188647	23.068045
102.476170	990.454485	23.073063
102.643468	986.449280	23.078080
102.558322	999.111050	23.083098
102.582479	983.530732	23.088115
102.819553	1004.426193	23.093133
103.196695	1006.643024	23.098151
103.471338	1010.860785	23.103168
103.421580	1009.063686	23.108186
103.536266	1010.068544	23.113203
103.655822	1011.826869	23.118221
103.575606	1009.488566	23.123239
103.372052	1015.068329	23.128256
103.630201	1010.089623	23.133274
103.765135	1008.929634	23.138291
103.793041	1026.108647	23.143309
104.347125	1022.197846	23.148327
104.379475	1028.132199	23.153344
104.695727	1024.940071	23.158362
105.065745	1014.001650	23.163379
104.875259	1022.779320	23.168397
104.948198	1018.842447	23.173415
104.874434	1008.096197	23.178432
104.939006	1008.474550	23.183450
105.269683	1013.693430	23.188467
105.076691	1016.346161	23.193485
104.985569	1010.765436	23.198503
105.041396	1010.646540	23.203520
104.928632	1013.873751	23.208538
105.346131	1029.174393	23.213555
105.672728	1038.272348	23.218573
105.572098	1037.571904	23.223591
105.901317	1029.221240	23.228608
105.639121	1031.307244	23.233626
105.864645	1026.273653	23.238643
105.882335	1044.827031	23.243661
106.185094	1047.424672	23.248679
106.707354	1044.004809	23.253696
106.490447	1047.803655	23.258714
106.677119	1036.107980	23.263731
106.670942	1037.939532	23.268749
107.108602	1033.055946	23.273767
107.157572	1038.299758	23.278784
107.189033	1037.449364	23.283802
107.477805	1027.552362	23.288819
107.267109	1037.986806	23.293837
107.597604	1029.014258	23.298855
107.553883	1029.273774	23.303872
107.118042	1036.454967	23.308890
107.977933	1040.663666	23.313907
107.917997	1054.293527	23.318925
108.071671	1051.420192	23.323943
108.131362	1054.068301	23.328960
108.193467	1054.456506	23.333978
108.553440	1048.631969	23.338995
108.503871	1045.597777	23.344013
108.435733	1045.009038	23.349031
108.339926	1044.083785	23.354048
108.317132	1045.100582	23.359066
108.850592	1040.921592	23.364083
108.566788	1045.743853	23.369101
108.468608	1049.136055	23.374119
108.849399	1051.784663	23.379136
108.982234	1060.183814	23.384154
109.395762	1062.458102	23.389171
109.363791	1065.770572	23.394189
109.319584	1061.432211	23.399207
109.528262	1045.772616	23.404224
109.110471	1047.466285	23.409242
109.708033	1053.634536	23.414259
110.070305	1066.346614	23.419277
110.105549	1072.062783	23.424295
110.227561	1060.992534	23.429312
109.723106	1073.479803	23.434330
110.237435	1063.885331	23.439347
110.662660	1061.831241	23.444365
110.736259	1064.717025	23.449383
110.761064	1063.044010	23.454400
110.643307	1070.683772	23.459418
111.073080	1064.031019	23.464435
111.178853	1073.235954	23.469453
111.581364	1080.636931	23.474471
111.523744	1072.715699	23.479488
111.436974	1083.907195	23.484506
111.663831	1076.648564	23.489523
111.931104	1074.858903	23.494541
111.849328	1073.707403	23.499559
112.083196	1078.124031	23.504576
111.813082	1079.113064	23.509594
111.870399	1073.449249	23.514611
111.950359	1075.605061	23.519629
111.864609	1074.690863	23.524647
112.217716	1075.974181	23.529664
112.386940	1087.618123	23.534682
112.579948	1087.673527	23.539699
112.563041	1101.328282	23.544717
112.413817	1092.452481	23.549735
112.808535	1081.396565	23.554752
112.691957	1094.811216	23.559770
113.096803	1096.477796	23.564787
113.875511	1091.575809	23.569805
114.057328	1097.524784	23.574823
114.330674	1084.237696	23.579840
114.040594	1085.750541	23.584858
114.020780	1078.022234	23.589875
114.180824	1069.486454	23.594893
114.068503	1077.169553	23.599911
114.358564	1064.501564	23.604928
114.248358	1070.524398	23.609946
114.452328	1083.564089	23.614963
114.342152	1090.385335	23.619981
114.182399	1093.354791	23.624999
114.461744	1088.413788	23.630016
114.473597	1085.878105	23.635034
114.647130	1082.272690	23.640051
115.053532	1091.755875	23.645069
115.064441	1098.391016	23.650087
115.460162	1102.255436	23.655104
114.858387	1113.628118	23.660122
115.291220	1111.367712	23.665139
115.248966	1099.265829	23.670157
115.450908	1116.149593	23.675175
116.137679	1121.038512	23.680192
115.992439	1125.602538	23.685210
116.018922	1121.003849	23.690227
116.277720	1115.403324	23.695245
116.477942	1130.160376	23.700263
116.834240	1122.509191	23.705280
116.593159	1118.741105	23.710298
116.721848	1106.959738	23.715315
116.475406	1114.985624	23.720333
116.508257	1113.926728	23.725351
117.117711	1111.345336	23.730368
117.178269	1116.120313	23.735386
116.683848	1107.219355	23.740403
116.639202	1102.256208	23.745421
116.705698	1128.988157	23.750439
117.279733	1132.575516	23.755456
117.384121	1128.494867	23.760474
117.420309	1137.893706	23.765491
117.644637	1147.058131	23.770509
117.549569	1155.779987	23.775527
118.241593	1139.256110	23.780544
118.668860	1147.928196	23.785562
118.598188	1143.193151	23.790579
118.512420	1139.953141	23.795597
118.530894	1144.520084	23.800615
118.783167	1135.272485	23.805632
118.654738	1149.042470	23.810650
118.916800	1155.764761	23.815667
119.479729	1160.161735	23.820685
119.137891	1160.455044	23.825703
119.522088	1158.473602	23.830720
119.194198	1157.212093	23.835738
119.343159	1145.579022	23.840755
119.622328	1141.433289	23.845773
119.723978	1153.539072	23.850791
120.205056	1158.030839	23.855808
120.255140	1160.197625	23.860826
120.413907	1163.218487	23.865843
120.389338	1167.782671	23.870861
120.728588	1161.260739	23.875879
120.831063	1154.371733	23.880896
120.938138	1153.487470	23.885914
120.837307	1155.529430	23.890931
120.903575	1156.380889	23.895949
120.588700	1156.281838	23.900967
120.586205	1160.599588	23.905984
120.507657	1175.469508	23.911002
120.982164	1181.114167	23.916019
121.309849	1175.023218	23.921037
121.359411	1182.517058	23.926055
121.796848	1186.068891	23.931072
122.220917	1182.093092	23.936090
122.655659	1188.895808	23.941107
123.425117	1192.074058	23.946125
122.592232	1184.841521	23.951143
122.727416	1150.656178	23.956160
122.885269	1148.227143	23.961178
122.818417	1145.056770	23.966195
122.988513	1138.488599	23.971213
122.708861	1154.667903	23.976231
123.012865	1137.267172	23.981248
123.035954	1144.168675	23.986266
122.980769	1154.070895	23.991283
123.245767	1163.714988	23.996301
123.333329	1166.952063	24.001319
123.463619	1163.542711	24.006336
123.320965	1166.137135	24.011354
123.786218	1167.816408	24.016371
123.673033	1177.860214	24.021389
123.733486	1189.271851	24.026407
124.061465	1186.885750	24.031424
124.103472	1188.504690	24.036442
123.921506	1193.055516	24.041459
124.433023	1197.722435	24.046477
124.601019	1200.924902	24.051495
125.077580	1202.908530	24.056512
125.065995	1205.703458	24.061530
125.128788	1209.010669	24.066547
125.237486	1195.891142	24.071565
125.540342	1198.996874	24.076583
125.688133	1191.854646	24.081600
125.572071	1194.157757	24.086618
125.613079	1202.486066	24.091635
125.554972	1186.321931	24.096653
125.179791	1197.814021	24.101671
126.057861	1202.228213	24.106688
125.989974	1205.196008	24.111706
126.435141	1206.155736	24.116723
126.795239	1204.430505	24.121741
126.689261	1215.905940	24.126759
127.019331	1210.631959	24.131776
126.897208	1202.354640	24.136794
126.580857	1212.897154	24.141811
126.979637	1205.337149	24.146829
127.122993	1217.133527	24.151847
127.481797	1220.782816	24.156864
127.455142	1219.237718	24.161882
127.324863	1222.133179	24.166899
127.661118	1222.052672	24.171917
127.602600	1223.412712	24.176935
127.777954	1214.259097	24.181952
128.064470	1226.282500	24.186970
128.031456	1233.599871	24.191987
128.808751	1233.996651	24.197005
128.351868	1230.057013	24.202023
128.438443	1235.272939	24.207040
128.415396	1234.008144	24.212058
128.655096	1242.649520	24.217075
129.302553	1239.522552	24.222093
129.314374	1239.836539	24.227111
129.183724	1237.259906	24.232128
129.684604	1247.167121	24.237146
129.780138	1249.030196	24.242163
130.024067	1242.362130	24.247181
129.952862	1240.183339	24.252199
129.866150	1234.967928	24.257216
130.090507	1228.896204	24.262234
130.221673	1229.311530	24.267251
130.326339	1236.039423	24.272269
130.186683	1243.764720	24.277287
130.594672	1253.566481	24.282304
130.759955	1247.425053	24.287322
130.775242	1251.730589	24.292339
131.154483	1255.424040	24.297357
131.044828	1254.545113	24.302375
131.073693	1252.252910	24.307392
131.364690	1246.328595	24.312410
131.432065	1250.111625	24.317427
131.885883	1259.281406	24.322445
131.990576	1263.386833	24.327463
132.004699	1260.809746	24.332480
132.273098	1256.394264	24.337498
132.096095	1251.218152	24.342515
132.031764	1255.848510	24.347533
132.210798	1258.616924	24.352551
132.558612	1258.780771	24.357568
132.508373	1248.718677	24.362586
132.614361	1267.368995	24.367603
132.808748	1275.840717	24.372621
132.797927	1269.183901	24.377639
133.351541	1266.159902	24.382656
133.249330	1269.022599	24.387674
133.476097	1276.129128	24.392691
133.679722	1258.415702	24.397709
133.704846	1267.248288	24.402727
133.475430	1263.023918	24.407744
134.036135	1268.311203	24.412762
134.244628	1282.839878	24.417779
134.232941	1272.560329	24.422797
134.573895	1289.447863	24.427815
134.440695	1285.325274	24.432832
134.751366	1286.965510	24.437850
134.868397	1279.891152	24.442867
135.028004	1268.404665	24.447885
134.999378	1281.079929	24.452903
135.116622	1273.364912	24.457920
135.044919	1270.252076	24.462938
135.174070	1288.838851	24.467955
135.562179	1284.022872	24.472973
135.570395	1292.832856	24.477991
135.774151	1286.212053	24.483008
136.172109	1292.111664	24.488026
136.370937	1306.272633	24.493043
136.420695	1296.677782	24.498061
136.316281	1300.945162	24.503079
136.534317	1306.673974	24.508096
137.160782	1294.609855	24.513114
136.763922	1298.228487	24.518131
137.126107	1294.723046	24.523149
136.947139	1295.609538	24.528167
137.170860	1298.749699	24.533184
137.350537	1306.024518	24.538202
137.270993	1308.738524	24.543219
137.873582	1315.303718	24.548237
137.997505	1310.298489	24.553255
138.038041	1316.364208	24.558272
138.362755	1313.700888	24.563290
138.200698	1312.246291	24.568307
138.515576	1307.195553	24.573325
138.134568	1305.449996	24.578343
138.416544	1313.945970	24.583360
138.748234	1321.320205	24.588378
138.711418	1331.099743	24.593395
139.080872	1326.984091	24.598413
138.965171	1321.268238	24.603431
138.862598	1332.130991	24.608448
139.657961	1330.315891	24.613466
139.490544	1349.428586	24.618483
140.241996	1330.711453	24.623501
140.311014	1326.289125	24.628519
139.929815	1332.199604	24.633536
140.435610	1325.478113	24.638554
139.577000	1339.781652	24.643571
140.064998	1332.886203	24.648589
140.398546	1349.399406	24.653607
141.132890	1350.768558	24.658624
141.569877	1344.812013	24.663642
141.143281	1350.915759	24.668659
141.336096	1342.415771	24.673677
141.296852	1342.914436	24.678695
141.149647	1354.371134	24.683712
141.644623	1343.378341	24.688730
141.470925	1351.493995	24.693747
141.448852	1358.557248	24.698765
141.756742	1356.142695	24.703783
142.092344	1358.274520	24.708800
142.451411	1360.380602	24.713818
142.301081	1355.597940	24.718835
142.230129	1364.896815	24.723853
142.922067	1370.561333	24.728871
142.886386	1381.495753	24.733888
143.410362	1379.978522	24.738906
143.142319	1379.736478	24.743923
143.371830	1370.669026	24.748941
143.529897	1365.917242	24.753959
143.493661	1370.038324	24.758976
143.584867	1364.504839	24.763994
143.753965	1366.820379	24.769011
144.023272	1364.474949	24.774029
144.150005	1364.351323	24.779047
144.039403	1371.775505	24.784064
144.229768	1372.251047	24.789082
144.212684	1378.332070	24.794099
144.658113	1375.637323	24.799117
144.964805	1376.700672	24.804135
145.162707	1379.664985	24.809152
145.111217	1366.103210	24.814170
145.763856	1382.705621	24.819187
145.724191	1384.258399	24.824205
145.583285	1389.749630	24.829223
145.786208	1387.386129	24.834240
145.951998	1384.113221	24.839258
145.733137	1387.022500	24.844275
145.825760	1385.938502	24.849293
146.180616	1387.057469	24.854311
146.410200	1400.768755	24.859328
146.370635	1396.767261	24.864346
146.715035	1408.305247	24.869363
146.625129	1395.752984	24.874381
146.822583	1387.410043	24.879399
147.054736	1413.760025	24.884416
147.402624	1417.253263	24.889434
147.754608	1412.341887	24.894451
147.837793	1403.792665	24.899469
148.301459	1408.334546	24.904487
148.342793	1409.382406	24.909504
148.746296	1393.319783	24.914522
148.697367	1396.051127	24.919539
149.023533	1395.445168	24.924557
149.071949	1397.536504	24.929575
148.584067	1397.454919	24.934592
148.773176	1390.170478	24.939610
148.884006	1392.943221	24.944627
149.119434	1391.117461	24.949645
149.082840	1395.737225	24.954663
148.674893	1408.417988	24.959680
149.283154	1404.994136	24.964698
149.759076	1416.300209	24.969715
149.979375	1415.177397	24.974733
150.278437	1423.377271	24.979751
150.339355	1423.380658	24.984768
150.781634	1421.446950	24.989786
150.828849	1428.938105	24.994803
150.640892	1420.147064	24.999821
151.171274	1419.136922	25.004839
150.803239	1425.878522	25.009856
151.186220	1421.527211	25.014874
150.404790	1415.457379	25.019891
150.983843	1423.553700	25.024909
151.146902	1432.604737	25.029927
151.474255	1433.488146	25.034944
151.710179	1433.031937	25.039962
151.944694	1440.105768	25.044979
152.213681	1451.488263	25.049997
152.531874	1455.917105	25.055015
152.400784	1456.117645	25.060032
152.765780	1460.113163	25.065050
153.006232	1449.317724	25.070067
152.821207	1446.011059	25.075085
153.195674	1442.629910	25.080103
153.316367	1449.670973	25.085120
153.180356	1438.293517	25.090138
153.220527	1444.239416	25.095155
153.252277	1445.392913	25.100173
153.819283	1452.970411	25.105191
153.715874	1466.774617	25.110208
153.773720	1463.073527	25.115226
153.877994	1462.255957	25.120243
154.062991	1473.058245	25.125261
154.778424	1476.153442	25.130279
154.907895	1477.206518	25.135296
155.072105	1481.391093	25.140314
155.003530	1476.289553	25.145331
155.026081	1473.995149	25.150349
155.198094	1473.498396	25.155367
155.331084	1484.435022	25.160384
155.534910	1493.564951	25.165402
156.179250	1492.565465	25.170419
156.153170	1490.076656	25.175437
156.083852	1495.455788	25.180455
156.215159	1491.339306	25.185472
156.236875	1485.788199	25.190490
156.334311	1498.008486	25.195507
156.480180	1498.610881	25.200525
157.197176	1502.024579	25.205543
156.931732	1501.472854	25.210560
157.438412	1504.420674	25.215578
157.571282	1508.960434	25.220595
157.872576	1513.148921	25.225613
158.255431	1515.715227	25.230631
157.868880	1516.624581	25.235648
158.359451	1514.096357	25.240666
158.393491	1515.599801	25.245683
158.222965	1523.765533	25.250701
158.192644	1506.839374	25.255719
158.231063	1521.432595	25.260736
158.508369	1522.405852	25.265754
159.257484	1526.496218	25.270771
159.286811	1531.213053	25.275789
159.624493	1526.887705	25.280807
159.478581	1527.806931	25.285824
159.850816	1530.201322	25.290842
159.847357	1523.593757	25.295859
159.900591	1522.266571	25.300877
160.180254	1516.173515	25.305895
160.541386	1538.419935	25.310912
160.664281	1535.926861	25.315930
160.493711	1533.896049	25.320947
160.265637	1536.349189	25.325965
160.590009	1534.014098	25.330983
160.824839	1544.335294	25.336000
161.453278	1543.470827	25.341018
161.674312	1547.542428	25.346035
161.413596	1553.159662	25.351053
161.819070	1549.915680	25.356071
162.000068	1544.525952	25.361088
161.913868	1550.466314	25.366106
162.273975	1552.278763	25.371123
162.133088	1554.923461	25.376141
162.509289	1554.751527	25.381159
162.740509	1553.661721	25.386176
162.743978	1553.547818	25.391194
163.244795	1549.187598	25.396211
163.090095	1550.325948	25.401229
163.276786	1551.332250	25.406247
163.273895	1557.941309	25.411264
163.413136	1565.168882	25.416282
163.816785	1560.227330	25.421299
163.504023	1556.407192	25.426317
163.903646	1568.085010	25.431335
164.087233	1575.728568	25.436352
164.342725	1577.506813	25.441370
164.553981	1576.079280	25.446387
164.436886	1574.835415	25.451405
164.829436	1570.675086	25.456423
164.976776	1576.058381	25.461440
165.418072	1593.290352	25.466458
165.714052	1588.851559	25.471475
165.842943	1591.507911	25.476493
166.139742	1591.430391	25.481511
166.019013	1594.024619	25.486528
166.325304	1586.743945	25.491546
166.435008	1584.290788	25.496563
166.181238	1581.360880	25.501581
166.336947	1590.785534	25.506599
166.411545	1604.565290	25.511616
166.675927	1611.918568	25.516634
166.907243	1596.936628	25.521651
166.964364	1616.541682	25.526669
167.264540	1618.066817	25.531687
167.766486	1621.968466	25.536704
167.794505	1619.449125	25.541722
167.916189	1622.813518	25.546739
168.181821	1628.740156	25.551757
168.406688	1632.015901	25.556775
168.906185	1631.180973	25.561792
168.911173	1634.241638	25.566810
169.443711	1622.807315	25.571827
169.069536	1629.764546	25.576845
169.382478	1633.825014	25.581863
169.293820	1629.465030	25.586880
169.150807	1625.429096	25.591898
169.615916	1626.969580	25.596915
169.821092	1630.860629	25.601933
170.160029	1631.130006	25.606951
170.448904	1633.417466	25.611968
170.622256	1634.126043	25.616986
170.184933	1632.212491	25.622003
170.673470	1629.529931	25.627021
170.665728	1641.769848	25.632039
171.256837	1650.937394	25.637056
171.315273	1655.703380	25.642074
171.406481	1649.762698	25.647091
171.270003	1652.788585	25.652109
171.227986	1659.463735	25.657127
171.692083	1658.968840	25.662144
172.007171	1669.028300	25.667162
172.247430	1665.519679	25.672180
172.351163	1661.735662	25.677197
171.978682	1674.720368	25.682215
172.418012	1676.851863	25.687232
172.560143	1687.736697	25.692250
173.206444	1678.642069	25.697268
173.251659	1700.641226	25.702285
173.744858	1701.931184	25.707303
173.910447	1693.750855	25.712320
174.258680	1703.502209	25.717338
174.551524	1689.511027	25.722356
174.524723	1688.672827	25.727373
174.621263	1686.209082	25.732391
174.893940	1678.065738	25.737408
174.595086	1698.445845	25.742426
174.780466	1683.243760	25.747444
175.089269	1678.250670	25.752461
174.833754	1683.497898	25.757479
175.132238	1681.362483	25.762496
174.670171	1688.216653	25.767514
175.343123	1698.236193	25.772532
175.503892	1713.836185	25.777549
175.431350	1701.659707	25.782567
176.060508	1713.800515	25.787584
176.352996	1724.945993	25.792602
176.828004	1730.502388	25.797620
176.643838	1733.785029	25.802637
176.387856	1731.395097	25.807655
177.052416	1737.644681	25.812672
176.834075	1734.090678	25.817690
177.305533	1738.606185	25.822708
177.404384	1743.520541	25.827725
178.227314	1749.218440	25.832743
178.472809	1743.607165	25.837760
178.326991	1751.592426	25.842778
178.628599	1750.504272	25.847796
178.606087	1747.727686	25.852813
178.589081	1740.150135	25.857831
178.827036	1738.910942	25.862848
178.833733	1741.337026	25.867866
179.405981	1752.287483	25.872884
179.302206	1756.087801	25.877901
179.530508	1760.874707	25.882919
180.044653	1755.007002	25.887936
179.771337	1763.498125	25.892954
180.293414	1763.830513	25.897972
180.772412	1763.996034	25.902989
180.811397	1767.183976	25.908007
181.407367	1750.623993	25.913024
181.064165	1761.568655	25.918042
181.138106	1763.179520	25.923060
181.008772	1758.115761	25.928077
181.412476	1756.778176	25.933095
181.545689	1755.094529	25.938112
181.470930	1764.697172	25.943130
181.761121	1765.030948	25.948148
182.127478	1774.337695	25.953165
182.067069	1768.521567	25.958183
182.398732	1779.739878	25.963200
182.574264	1789.388776	25.968218
183.113925	1789.058844	25.973236
183.198412	1786.931487	25.978253
182.925570	1791.039009	25.983271
183.644109	1800.341433	25.988288
183.458297	1809.046179	25.993306
183.695478	1802.296900	25.998324
184.029055	1805.407425	26.003341
183.809488	1811.999819	26.008359
184.251262	1803.725946	26.013376
185.037284	1824.170829	26.018394
184.921195	1815.961712	26.023412
184.969907	1808.910404	26.028429
185.039094	1811.033269	26.033447
185.503674	1805.567753	26.038464
185.198838	1807.890865	26.043482
185.870679	1823.203095	26.048500
186.116579	1823.657380	26.053517
186.130883	1824.794682	26.058535
186.224435	1823.177165	26.063552
186.204623	1828.280438	26.068570
186.418863	1824.359257	26.073588
186.431738	1819.573152	26.078605
186.886743	1839.261678	26.083623
187.460336	1836.430141	26.088640
187.233888	1844.566856	26.093658
187.437024	1826.650961	26.098676
187.135169	1837.788054	26.103693
187.681235	1841.809120	26.108711
188.156167	1839.002411	26.113728
188.120630	1853.276049	26.118746
188.627115	1843.707627	26.123764
188.663271	1851.484714	26.128781
188.403217	1847.138738	26.133799
188.553345	1851.909436	26.138816
188.720604	1872.759990	26.143834
188.959891	1867.594627	26.148852
189.513066	1878.617562	26.153869
189.621104	1895.589278	26.158887
190.168869	1885.944978	26.163904
190.165035	1886.299285	26.168922
190.265494	1878.798064	26.173940
190.418741	1879.904270	26.178957
190.741806	1895.920983	26.183975
191.281458	1888.155714	26.188992
191.191278	1897.315845	26.194010
191.308307	1891.165928	26.199028
191.359341	1888.040187	26.204045
191.063395	1900.413517	26.209063
191.680605	1894.135232	26.214080
192.330053	1906.077347	26.219098
192.356263	1900.115142	26.224116
192.748431	1905.185855	26.229133
192.844750	1907.465460	26.234151
193.087797	1899.288756	26.239168
192.942655	1915.113284	26.244186
193.568132	1927.018118	26.249204
194.102581	1921.746824	26.254221
193.862121	1920.402215	26.259239
194.017052	1916.644888	26.264256
193.684312	1922.904635	26.269274
193.960506	1923.417325	26.274292
194.355876	1925.303221	26.279309
194.570396	1937.120560	26.284327
195.033963	1941.867731	26.289344
195.213668	1932.911893	26.294362
195.670566	1918.219622	26.299380
195.449367	1908.126963	26.304397
195.690791	1911.128773	26.309415
196.091671	1913.783855	26.314432
195.907105	1929.614534	26.319450
196.294393	1943.816103	26.324468
196.562986	1929.759078	26.329485
196.637869	1930.997412	26.334503
196.676634	1922.205539	26.339520
196.990785	1926.079687	26.344538
196.741590	1943.268018	26.349556
197.199774	1945.721672	26.354573
197.197012	1950.999057	26.359591
197.497476	1956.327069	26.364608
197.681987	1960.899932	26.369626
197.545558	1962.076490	26.374644
197.863747	1972.659524	26.379661
198.269987	1972.530250	26.384679
198.600912	1971.781516	26.389696
198.393450	1990.339381	26.394714
198.857873	1998.103506	26.399732
199.498069	1996.890038	26.404749
199.311703	1998.961191	26.409767
199.596421	1997.651581	26.414784
199.905347	2001.914739	26.419802
200.194271	2011.691278	26.424820
200.581585	2007.004622	26.429837
200.535692	2012.421290	26.434855
200.524425	2010.286723	26.439872
201.078221	2000.852869	26.444890
200.590639	2005.483043	26.449908
201.551263	2009.142947	26.454925
201.437729	2015.728375	26.459943
201.734986	2023.411236	26.464960
201.992520	2020.344844	26.469978
201.895883	2018.630683	26.474996
202.228714	2008.511673	26.480013
202.317864	2023.425626	26.485031
202.529761	2026.368934	26.490048
202.692931	2042.783074	26.495066
202.928433	2037.293190	26.500084
203.182548	2043.212293	26.505101
203.465960	2048.382034	26.510119
203.858667	2056.274121	26.515136
204.088114	2048.759059	26.520154
204.128864	2057.851550	26.525172
203.948704	2055.856885	26.530189
204.172273	2073.808064	26.535207
204.479219	2071.548204	26.540224
204.362258	2075.770384	26.545242
204.948895	2085.730997	26.550260
205.501358	2090.555891	26.555277
205.524121	2093.632803	26.560295
205.674979	2101.467884	26.565312
206.278090	2109.980520	26.570330
206.420541	2108.494227	26.575348
206.586075	2112.473609	26.580365
206.508080	2117.175749	26.585383
206.902448	2108.047540	26.590400
206.857225	2122.834167	26.595418
206.764460	2127.939415	26.600436
207.063060	2124.809804	26.605453
207.580149	2143.406510	26.610471
207.846045	2140.556556	26.615488
208.366480	2145.181315	26.620506
208.432273	2143.397669	26.625524
208.451164	2138.364376	26.630541
208.387769	2145.573238	26.635559
208.892059	2150.351998	26.640576
209.216335	2155.439665	26.645594
209.192164	2157.472960	26.650612
209.485896	2161.088394	26.655629
209.693924	2174.355489	26.660647
209.893139	2174.611914	26.665664
210.408414	2176.924161	26.670682
210.007817	2173.796096	26.675700
210.245401	2187.513057	26.680717
210.834251	2194.367915	26.685735
210.837614	2197.466801	26.690752
211.000982	2204.716126	26.695770
211.375690	2216.713849	26.700788
211.843274	2215.647168	26.705805
211.542112	2216.751554	26.710823
212.064235	2228.518040	26.715840
212.574199	2224.967320	26.720858
212.286295	2231.264378	26.725876
212.774712	2226.672384	26.730893
212.481016	2223.126858	26.735911
212.604345	2232.253920	26.740928
213.016780	2239.079453	26.745946
213.028132	2246.339838	26.750964
213.310185	2257.471496	26.755981
213.616362	2266.633228	26.760999
213.974776	2267.521314	26.766016
214.344885	2271.374202	26.771034
214.707502	2273.072721	26.776052
214.978680	2269.319314	26.781069
215.122516	2271.717807	26.786087
215.451463	2273.481532	26.791104
215.389801	2255.795791	26.796122
215.328590	2267.416423	26.801140
215.762946	2280.761975	26.806157
215.832879	2289.771141	26.811175
216.073798	2284.621184	26.816192
216.385005	2282.016632	26.821210
216.394788	2303.343514	26.826228
216.948255	2306.653437	26.831245
216.919295	2303.050899	26.836263
217.250371	2306.777320	26.841280
217.499672	2314.862272	26.846298
217.552743	2325.887603	26.851316
217.972827	2317.433823	26.856333
217.947944	2334.174172	26.861351
218.271393	2341.158774	26.866368
218.614633	2335.560502	26.871386
218.777996	2358.258487	26.876404
219.296290	2356.723128	26.881421
219.518612	2362.634663	26.886439
219.289026	2363.475435	26.891456
219.988407	2364.439837	26.896474
219.913417	2387.547376	26.901492
220.068837	2375.353883	26.906509
220.404193	2376.958820	26.911527
220.444572	2398.157967	26.916544
220.649502	2403.074926	26.921562
220.721747	2401.678440	26.926580
221.282889	2401.234696	26.931597
221.623814	2428.557079	26.936615
221.280115	2431.574331	26.941632
221.914962	2418.491916	26.946650
222.277432	2442.367761	26.951668
222.611478	2457.098772	26.956685
222.387478	2447.189292	26.961703
222.598495	2459.648194	26.966720
223.353222	2460.717602	26.971738
223.364873	2467.381543	26.976756
223.963338	2458.940953	26.981773
224.302957	2465.317132	26.986791
224.028280	2468.052226	26.991808
224.615352	2465.903351	26.996826
224.597531	2464.019075	27.001844
225.059337	2473.286081	27.006861
225.215824	2471.822821	27.011879
225.254893	2472.501842	27.016896
225.488344	2475.239885	27.021914
225.452782	2483.552312	27.026932
225.723419	2485.839568	27.031949
225.839248	2496.271370	27.036967
225.785142	2499.890531	27.041984
226.262735	2507.371944	27.047002
226.488005	2505.689676	27.052020
226.451550	2523.501896	27.057037
227.119986	2519.554035	27.062055
227.522478	2527.899277	27.067072
227.920529	2529.273546	27.072090
228.109564	2534.499151	27.077108
228.421981	2520.513740	27.082125
228.607685	2522.116742	27.087143
228.788327	2529.344573	27.092160
228.630233	2520.882876	27.097178
228.898662	2533.165621	27.102196
228.992173	2538.955249	27.107213
229.460059	2548.511703	27.112231
229.084453	2553.818909	27.117248
230.264050	2551.139086	27.122266
229.888983	2559.434973	27.127284
230.349787	2565.161114	27.132301
230.367102	2576.567734	27.137319
230.091137	2578.217369	27.142336
230.578922	2589.121530	27.147354
230.590788	2602.855017	27.152372
230.886812	2609.664100	27.157389
231.109612	2618.504454	27.162407
231.313424	2636.607608	27.167424
231.767577	2632.071343	27.172442
231.960302	2649.421942	27.177460
232.483038	2658.143030	27.182477
232.603109	2663.098521	27.187495
233.001193	2678.996952	27.192512
233.332859	2674.312477	27.197530
233.467218	2679.833837	27.202548
233.963330	2679.671633	27.207565
234.403717	2699.678993	27.212583
234.165611	2705.097391	27.217600
234.436394	2691.474964	27.222618
234.206584	2707.297593	27.227636
234.819641	2713.880619	27.232653
235.024792	2711.958447	27.237671
235.091248	2726.008603	27.242688
235.525855	2739.796309	27.247706
235.902134	2744.033380	27.252724
235.657728	2758.832605	27.257741
236.029202	2760.895897	27.262759
236.658897	2774.069384	27.267776
237.280114	2776.990121	27.272794
237.361660	2785.076155	27.277812
237.437240	2786.020926	27.282829
237.715859	2783.093146	27.287847
237.644656	2798.828040	27.292864
238.097038	2796.362397	27.297882
238.207094	2795.856319	27.302900
238.766939	2806.247578	27.307917
239.132069	2816.937425	27.312935
239.065156	2816.165383	27.317952
239.553955	2807.085241	27.322970
239.748969	2811.517821	27.327988
239.869906	2820.749707	27.333005
240.309497	2824.377285	27.338023
240.096046	2830.183236	27.343040
240.643060	2826.178469	27.348058
240.269622	2838.034288	27.353076
241.007643	2843.294445	27.358093
241.007496	2844.415125	27.363111
241.257282	2856.947170	27.368128
241.664525	2853.491223	27.373146
241.643383	2871.102571	27.378164
242.054914	2886.285818	27.383181
242.402009	2883.558818	27.388199
242.714315	2890.627430	27.393216
242.878721	2889.424860	27.398234
243.182770	2905.079333	27.403252
242.946506	2897.576456	27.408269
243.530067	2908.349127	27.413287
243.925199	2927.196032	27.418304
243.859598	2928.509961	27.423322
244.292831	2941.442735	27.428340
244.433249	2952.432760	27.433357
244.932960	2950.057566	27.438375
244.686699	2954.401078	27.443392
245.008429	2964.700101	27.448410
244.925774	2978.262380	27.453428
245.250774	2983.520602	27.458445
245.614470	2992.604319	27.463463
246.024740	2997.470537	27.468480
246.389388	3005.509439	27.473498
246.800221	3022.110004	27.478516
246.564329	3026.713876	27.483533
246.719600	3027.501071	27.488551
246.847841	3044.634851	27.493568
247.229620	3047.987426	27.498586
248.146148	3050.937979	27.503604
248.063679	3066.696955	27.508621
248.649477	3071.526398	27.513639
248.727486	3083.267909	27.518656
248.875027	3079.161160	27.523674
249.011632	3086.427634	27.528692
249.717709	3097.998782	27.533709
249.887211	3104.616291	27.538727
249.979103	3113.448865	27.543744
250.086266	3111.242075	27.548762
250.371244	3116.629656	27.553780
250.534438	3129.437332	27.558797
250.873588	3136.202029	27.563815
250.985397	3151.059739	27.568832
251.112303	3146.227120	27.573850
251.284911	3162.492480	27.578868
251.959941	3169.956058	27.583885
252.257688	3172.100313	27.588903
252.347524	3183.761144	27.593920
252.639806	3182.478679	27.598938
252.677192	3202.606154	27.603956
252.456193	3221.126367	27.608973
253.544036	3224.798287	27.613991
253.830902	3233.707875	27.619008
254.191508	3232.073905	27.624026
254.279892	3241.497288	27.629044
254.777027	3250.538268	27.634061
254.768137	3246.427431	27.639079
255.214354	3258.086481	27.644096
255.241216	3278.048402	27.649114
255.766391	3272.374173	27.654132
255.360177	3283.077077	27.659149
256.177519	3291.607426	27.664167
256.192836	3299.300014	27.669184
256.192498	3304.230243	27.674202
257.191119	3317.734903	27.679220
257.283423	3316.107979	27.684237
257.328666	3319.453032	27.689255
257.732247	3335.389065	27.694272
258.244433	3336.632008	27.699290
258.114520	3336.693512	27.704308
258.184174	3354.865620	27.709325
258.640610	3361.530081	27.714343
259.029117	3370.332384	27.719360
259.228249	3366.567874	27.724378
259.705732	3373.790863	27.729396
259.492569	3391.407365	27.734413
259.771559	3386.942371	27.739431
260.403580	3397.117586	27.744448
260.195220	3404.270618	27.749466
260.646145	3412.968538	27.754484
260.953782	3421.287935	27.759501
261.218029	3427.666724	27.764519
261.280634	3443.438162	27.769536
262.052704	3434.979560	27.774554
262.201377	3433.558471	27.779572
261.867620	3443.549515	27.784589
262.566861	3454.099353	27.789607
262.451704	3451.857697	27.794624
262.979630	3464.507830	27.799642
263.431664	3475.285539	27.804660
263.226387	3481.623823	27.809677
263.479589	3480.738790	27.814695
263.601148	3498.830370	27.819712
264.063217	3506.469274	27.824730
264.454465	3523.313224	27.829748
264.763514	3527.321078	27.834765
264.835071	3534.405332	27.839783
264.791171	3555.095035	27.844800
265.014002	3556.020079	27.849818
265.230306	3573.431023	27.854836
265.630445	3585.782359	27.859853
265.959240	3592.094346	27.864871
266.546558	3614.563793	27.869888
266.326937	3618.723411	27.874906
267.222116	3629.189192	27.879924
267.535222	3643.523599	27.884941
268.169392	3637.665008	27.889959
268.161754	3652.267137	27.894976
268.243021	3653.864408	27.899994
268.609931	3653.390911	27.905012
268.952477	3676.359352	27.910029
269.285434	3682.071039	27.915047
269.641765	3684.329328	27.920064
269.596860	3690.311313	27.925082
270.026672	3696.484517	27.930100
270.146471	3704.602884	27.935117
270.695230	3722.776523	27.940135
270.733799	3731.333641	27.945152
270.731873	3733.439400	27.950170
271.087855	3741.757731	27.955188
271.442974	3752.661164	27.960205
271.954181	3762.148398	27.965223
271.914267	3772.507345	27.970240
271.953357	3787.522089	27.975258
272.593855	3797.112307	27.980276
272.878895	3813.588001	27.985293
273.296860	3810.464769	27.990311
273.796420	3817.324687	27.995328
273.699932	3835.813522	28.000346
274.089170	3842.785313	28.005364
273.758144	3850.487869	28.010381
273.972228	3853.282796	28.015399
274.331143	3866.464527	28.020416
274.975898	3888.344622	28.025434
275.354664	3895.690504	28.030452
275.657504	3910.651664	28.035469
276.323584	3907.464536	28.040487
276.670639	3922.513510	28.045504
276.891251	3929.833528	28.050522
277.080685	3908.423698	28.055540
277.565815	3928.087741	28.060557
277.845742	3933.586826	28.065575
278.073050	3946.164162	28.070592
278.029054	3952.679503	28.075610
278.366865	3953.002755	28.080628
278.255101	3980.606292	28.085645
278.711756	3970.425875	28.090663
278.991925	3967.942700	28.095680
278.838205	3991.370714	28.100698
279.330919	4001.877278	28.105716
279.481808	4008.693709	28.110733
279.744968	4015.584195	28.115751
280.378996	4034.306693	28.120768
280.379236	4042.582703	28.125786
280.861657	4058.036815	28.130804
280.825034	4066.523735	28.135821
281.005040	4079.193748	28.140839
281.094482	4084.814067	28.145856
281.541399	4107.410146	28.150874
282.394246	4113.306161	28.155892
282.270281	4124.584255	28.160909
282.655221	4133.542147	28.165927
283.262618	4141.676332	28.170944
283.248904	4157.712780	28.175962
283.644971	4160.280575	28.180980
283.834528	4174.644109	28.185997
284.044392	4182.685544	28.191015
284.785129	4187.989868	28.196032
284.738305	4203.589628	28.201050
285.187949	4200.603432	28.206068
285.281295	4219.422924	28.211085
285.771041	4229.895364	28.216103
285.960461	4231.463223	28.221120
286.003287	4255.946757	28.226138
286.374225	4257.985059	28.231156
286.276064	4280.451585	28.236173
286.940008	4281.181739	28.241191
287.333260	4293.465194	28.246208
287.682795	4302.952634	28.251226
288.381245	4311.410449	28.256244
288.512613	4316.774962	28.261261
288.752596	4326.746609	28.266279
289.003379	4345.983611	28.271296
289.119972	4352.606660	28.276314
289.232299	4355.332287	28.281332
289.721279	4367.787114	28.286349
289.849393	4393.807323	28.291367
290.272766	4391.301796	28.296384
290.730897	4403.085990	28.301402
291.738979	4402.739913	28.306420
291.563942	4399.765717	28.311437
291.707156	4409.092797	28.316455
292.136130	4417.684150	28.321472
291.875223	4428.267259	28.326490
292.913931	4437.625382	28.331508
292.861567	4455.514583	28.336525
292.955451	4456.333495	28.341543
293.369498	4457.916905	28.346560
293.477832	4475.490722	28.351578
293.817713	4484.159105	28.356596
293.967777	4497.578977	28.361613
294.510792	4516.445558	28.366631
295.063298	4525.551158	28.371648
294.591227	4531.486294	28.376666
295.362726	4547.795390	28.381684
295.796653	4560.000097	28.386701
295.390516	4563.311493	28.391719
296.037586	4571.916312	28.396736
296.106319	4597.317938	28.401754
296.670629	4610.689184	28.406772
296.902806	4617.430061	28.411789
297.066023	4633.486731	28.416807
297.638676	4640.894269	28.421824
297.801309	4662.834582	28.426842
297.966360	4678.225005	28.431860
298.352524	4682.438905	28.436877
298.956417	4693.392556	28.441895
299.342083	4710.181669	28.446912
299.249046	4720.672529	28.451930
299.610222	4739.716003	28.456948
300.278955	4731.601160	28.461965
300.279007	4744.968816	28.466983
300.903859	4754.312626	28.472000
300.867713	4768.913781	28.477018
300.877485	4763.912739	28.482036
301.133460	4774.298791	28.487053
301.166624	4800.751015	28.492071
301.669181	4808.617747	28.497088
302.145208	4830.537881	28.502106
302.755099	4836.806543	28.507124
302.673124	4867.184452	28.512141
302.728492	4877.952159	28.517159
303.294981	4890.433157	28.522176
303.639765	4916.982233	28.527194
303.954862	4929.382451	28.532212
303.971214	4944.016607	28.537229
304.302324	4958.475514	28.542247
304.974829	4962.139869	28.547264
305.492001	4980.666904	28.552282
305.757021	4987.551159	28.557300
306.066322	5005.334093	28.562317
306.060309	5027.616750	28.567335
306.791880	5027.200082	28.572352
307.071223	5042.311035	28.577370
306.994048	5046.578216	28.582388
307.857265	5064.540116	28.587405
308.045304	5072.986216	28.592423
308.160080	5083.479652	28.597440
308.645244	5097.232888	28.602458
308.858405	5108.809476	28.607476
309.413150	5118.663114	28.612493
309.289349	5131.725219	28.617511
309.724625	5137.222581	28.622528
309.970578	5154.598868	28.627546
310.162327	5163.773582	28.632564
310.366363	5196.178170	28.637581
310.813688	5200.733040	28.642599
311.693140	5215.839092	28.647616
311.883477	5229.985543	28.652634
312.069396	5248.466572	28.657652
312.136460	5248.494257	28.662669
312.782215	5275.060129	28.667687
313.570066	5273.173233	28.672704
313.360978	5285.529043	28.677722
313.176394	5297.322342	28.682740
313.697742	5308.399697	28.687757
314.014771	5329.830676	28.692775
314.770385	5337.550921	28.697792
314.803373	5354.714346	28.702810
315.116470	5366.436523	28.707828
315.287126	5371.075545	28.712845
315.717533	5391.267370	28.717863
316.153631	5386.575412	28.722880
316.273880	5406.285244	28.727898
316.860593	5419.126461	28.732916
317.220339	5435.737203	28.737933
317.242214	5448.117139	28.742951
317.724417	5468.910199	28.747968
317.812466	5472.419439	28.752986
318.301505	5487.472864	28.758004
318.429716	5504.122871	28.763021
318.686005	5520.787676	28.768039
319.038889	5527.118688	28.773056
319.422825	5538.659494	28.778074
319.960730	5555.027963	28.783092
319.982800	5572.594176	28.788109
320.582010	5587.475860	28.793127
321.275096	5578.817081	28.798144
321.669366	5593.064642	28.803162
321.864267	5603.034541	28.808180
322.248543	5610.904255	28.813197
322.242755	5615.801239	28.818215
322.425025	5620.807835	28.823232
322.675047	5628.793155	28.828250
322.760348	5641.018146	28.833268
323.135761	5646.253519	28.838285
323.374835	5667.775947	28.843303
324.006799	5669.906351	28.848320
324.065129	5689.556686	28.853338
324.440501	5704.953115	28.858356
325.209588	5722.037010	28.863373
325.533149	5735.373968	28.868391
326.134293	5736.132906	28.873408
326.475672	5741.275751	28.878426
326.369763	5754.547007	28.883444
326.947080	5762.661358	28.888461
326.964840	5777.488518	28.893479
327.313228	5789.196004	28.898496
327.647282	5798.705579	28.903514
327.561740	5811.329760	28.908532
327.877053	5820.804386	28.913549
328.050465	5848.038075	28.918567
328.454648	5866.498378	28.923584
329.011661	5876.216342	28.928602
329.229106	5905.640264	28.933620
329.743022	5920.305068	28.938637
330.357386	5932.166948	28.943655
330.797170	5945.678520	28.948672
330.917585	5964.432474	28.953690
330.978874	5983.527098	28.958708
331.487656	5995.392831	28.963725
331.482566	6009.185204	28.968743
331.999711	6033.054346	28.973760
332.529939	6049.841133	28.978778
333.012888	6063.001998	28.983796
333.444028	6065.514103	28.988813
333.140407	6093.027606	28.993831
334.043484	6107.609878	28.998848
334.150725	6121.416414	29.003866
334.739585	6138.648714	29.008884
335.022038	6148.693668	29.013901
335.260725	6160.730981	29.018919
335.606127	6171.580566	29.023936
336.068866	6186.158852	29.028954
336.206458	6200.579430	29.033972
337.220807	6196.744242	29.038989
337.357828	6209.949599	29.044007
337.514870	6227.062966	29.049024
337.967746	6233.075617	29.054042
338.075189	6252.699972	29.059060
338.536201	6258.092657	29.064077
338.988024	6268.146032	29.069095
339.120535	6279.439194	29.074112
339.364916	6303.682607	29.079130
339.766575	6313.516536	29.084148
340.039183	6327.401654	29.089165
340.064387	6341.492604	29.094183
340.677870	6353.465381	29.099200
341.199416	6358.937060	29.104218
340.934182	6379.115171	29.109236
341.461105	6383.910486	29.114253
341.938934	6407.139116	29.119271
342.592766	6429.330228	29.124288
343.005082	6446.164148	29.129306
343.323636	6459.928572	29.134324
343.610479	6459.072888	29.139341
343.960185	6473.353331	29.144359
344.179728	6481.249069	29.149376
344.582801	6498.352798	29.154394
344.727192	6511.838174	29.159412
344.982918	6523.910955	29.164429
344.647420	6534.743649	29.169447
345.474819	6553.927942	29.174464
345.963678	6566.052845	29.179482
346.101844	6579.340366	29.184500
347.283686	6589.236073	29.189517
347.635208	6594.964735	29.194535
347.693383	6598.646150	29.199552
347.963143	6615.890700	29.204570
348.034627	6627.900687	29.209588
348.820808	6640.358160	29.214605
348.897926	6658.895439	29.219623
348.921072	6670.673067	29.224640
349.136731	6674.557267	29.229658
349.675936	6702.429767	29.234676
349.766760	6727.003853	29.239693
350.123724	6742.868069	29.244711
350.745884	6765.853713	29.249728
350.836942	6788.031859	29.254746
351.139487	6813.469622	29.259764
351.546355	6824.941382	29.264781
352.180161	6854.447224	29.269799
352.297589	6871.911450	29.274816
352.822900	6894.356739	29.279834
352.959663	6913.248019	29.284852
353.599743	6936.644627	29.289869
354.540916	6948.124829	29.294887
355.449061	6954.701360	29.299904
355.458211	6946.874482	29.304922
355.769608	6974.350382	29.309940
356.154820	6971.048624	29.314957
356.459936	6980.856906	29.319975
356.908355	6999.731324	29.324992
357.317763	7005.290106	29.330010
357.122989	7025.375881	29.335028
357.274470	7029.415361	29.340045
357.640486	7061.510773	29.345063
357.808448	7067.539647	29.350080
358.276834	7090.227643	29.355098
358.579420	7111.533536	29.360116
359.236300	7136.960780	29.365133
359.571809	7146.458206	29.370151
359.592505	7170.213557	29.375168
360.383525	7187.882588	29.380186
360.870708	7199.361021	29.385204
361.206802	7209.837010	29.390221
361.540058	7229.206277	29.395239
362.058720	7236.695895	29.400256
362.759722	7246.376392	29.405274
362.914722	7263.115381	29.410292
363.543110	7268.580172	29.415309
363.894247	7281.999203	29.420327
363.625549	7294.681332	29.425344
364.161458	7315.076687	29.430362
364.149553	7322.128058	29.435380
364.689968	7335.656563	29.440397
365.070501	7357.616705	29.445415
365.210054	7371.589625	29.450432
365.868548	7390.403330	29.455450
365.937435	7414.482966	29.460468
366.311847	7432.179210	29.465485
366.795251	7452.747050	29.470503
367.111027	7474.288077	29.475520
367.620424	7487.903603	29.480538
367.703967	7500.897234	29.485556
368.486413	7507.263083	29.490573
368.980738	7522.295269	29.495591
369.267608	7530.468258	29.500608
369.836353	7533.682076	29.505626
370.046781	7553.863190	29.510644
370.032036	7562.092619	29.515661
370.461870	7579.174251	29.520679
370.283061	7595.179441	29.525696
370.818249	7609.334031	29.530714
370.779277	7627.849321	29.535732
371.469512	7662.556588	29.540749
371.890168	7678.275952	29.545767
372.562366	7693.315313	29.550784
373.075433	7710.125242	29.555802
373.536083	7739.353244	29.560820
373.444507	7747.711524	29.565837
373.982378	7774.957634	29.570855
373.912192	7789.212923	29.575872
374.491204	7807.300706	29.580890
374.950037	7832.021022	29.585908
375.495377	7848.627165	29.590925
375.361336	7867.293246	29.595943
376.016916	7897.580302	29.600960
376.641452	7910.619436	29.605978
376.963447	7937.769960	29.610996
377.705941	7947.775853	29.616013
378.338346	7968.889330	29.621031
378.509615	7975.416790	29.626048
379.202902	7990.140571	29.631066
379.452431	8013.413096	29.636084
379.617607	8020.977009	29.641101
380.377822	8035.873513	29.646119
380.380188	8049.764125	29.651136
381.027436	8059.437639	29.656154
381.406377	8075.640543	29.661172
381.699149	8097.779397	29.666189
382.284995	8107.178366	29.671207
382.240333	8128.277467	29.676224
383.057662	8137.687769	29.681242
383.072766	8156.981266	29.686260
383.282858	8169.715736	29.691277
384.122891	8190.768731	29.696295
384.163375	8201.761703	29.701312
384.268786	8217.783168	29.706330
384.901184	8241.529910	29.711348
385.181120	8264.261324	29.716365
385.279749	8273.262676	29.721383
385.896327	8309.141259	29.726400
386.504119	8320.349057	29.731418
386.948040	8327.345634	29.736436
387.763670	8343.626013	29.741453
388.356504	8353.882735	29.746471
388.631364	8364.258420	29.751488
388.951345	8380.038257	29.756506
389.077245	8392.615508	29.761524
389.377254	8405.020438	29.766541
389.470893	8419.717952	29.771559
389.684077	8443.653344	29.776576
390.639857	8450.289303	29.781594
390.774657	8470.587379	29.786612
391.556498	8491.428785	29.791629
392.035220	8503.474467	29.796647
392.242181	8519.919217	29.801664
392.802319	8524.397380	29.806682
392.768738	8532.551248	29.811700
393.016599	8555.550052	29.816717
393.403875	8569.712625	29.821735
393.727396	8599.443217	29.826752
394.373518	8598.806172	29.831770
394.697183	8616.887150	29.836788
394.943736	8630.711770	29.841805
395.384434	8651.912705	29.846823
395.333452	8663.128559	29.851840
395.823170	8684.511325	29.856858
395.944980	8711.283732	29.861876
396.440557	8739.178746	29.866893
396.797336	8757.519902	29.871911
397.004368	8782.624821	29.876928
397.676087	8799.010094	29.881946
398.224736	8826.499181	29.886964
398.442745	8851.741398	29.891981
398.873934	8878.251197	29.896999
399.377672	8908.071044	29.902016
400.033488	8921.753239	29.907034
400.262955	8942.526450	29.912052
400.611826	8966.618196	29.917069
401.320109	8986.035114	29.922087
401.447296	9006.780121	29.927104
402.109322	9020.707681	29.932122
402.963441	9038.845404	29.937140
402.828160	9052.448798	29.942157
403.243323	9085.509335	29.947175
403.525794	9102.154377	29.952192
404.284022	9117.996062	29.957210
404.713830	9132.496577	29.962228
405.157034	9153.877657	29.967245
405.352208	9179.341721	29.972263
405.396216	9199.809433	29.977280
405.484952	9225.400631	29.982298
406.505453	9246.871904	29.987316
407.139244	9269.050630	29.992333
407.630791	9278.471196	29.997351
407.906860	9303.856535	30.002368
408.610216	9318.598759	30.007386
408.855959	9338.369047	30.012404
409.449267	9358.315725	30.017421
409.833349	9374.645258	30.022439
410.178250	9395.129487	30.027456
410.808581	9404.307506	30.032474
411.393402	9427.513827	30.037492
411.342002	9450.711879	30.042509
411.665127	9465.210321	30.047527
411.668349	9481.681329	30.052544
411.927065	9497.389570	30.057562
412.732570	9524.694476	30.062580
413.041529	9547.583969	30.067597
413.592547	9567.635330	30.072615
413.731284	9591.245971	30.077632
414.577108	9612.564901	30.082650
414.894357	9638.184239	30.087668
414.921466	9670.580063	30.092685
415.916418	9684.266859	30.097703
416.340907	9707.312213	30.102720
416.710489	9718.138032	30.107738
417.406409	9732.158728	30.112756
417.442010	9760.439461	30.117773
418.306061	9764.854831	30.122791
418.963288	9789.139595	30.127808
418.966959	9799.994011	30.132826
419.444622	9820.514872	30.137844
419.735313	9832.991672	30.142861
420.413213	9848.972783	30.147879
420.218165	9866.482176	30.152896
420.387422	9890.404175	30.157914
420.715045	9908.807843	30.162932
420.960972	9941.110084	30.167949
422.030927	9965.501320	30.172967
422.410761	9973.859832	30.177984
422.941666	9985.288998	30.183002
423.120406	10006.336513	30.188020
423.991092	10024.557875	30.193037
424.091306	10040.509107	30.198055
424.402060	10060.491058	30.203072
424.957931	10071.329127	30.208090
425.727346	10092.635247	30.213108
425.702665	10115.580539	30.218125
425.777502	10125.451606	30.223143
426.207410	10154.647170	30.228160
426.934116	10183.307186	30.233178
427.247737	10202.925748	30.238196
427.552945	10228.219409	30.243213
428.316743	10257.991470	30.248231
428.534040	10278.723869	30.253248
429.080729	10294.009069	30.258266
429.590650	10323.419773	30.263284
429.965244	10350.439353	30.268301
430.317397	10357.779358	30.273319
430.735189	10385.919449	30.278336
430.965472	10408.569661	30.283354
431.346621	10434.066482	30.288372
431.752203	10463.250530	30.293389
432.338851	10486.577874	30.298407
432.679493	10508.585861	30.303424
433.304224	10542.408875	30.308442
433.716607	10568.510398	30.313460
434.067857	10587.750932	30.318477
434.836178	10618.397471	30.323495
435.619530	10638.720090	30.328512
435.841505	10667.702551	30.333530
436.401880	10681.183046	30.338548
436.499199	10699.721231	30.343565
437.248975	10721.144798	30.348583
437.685675	10739.598614	30.353600
437.953619	10760.945682	30.358618
438.973021	10769.514415	30.363636
439.372990	10789.577982	30.368653
439.913508	10804.826674	30.373671
440.233228	10812.718147	30.378688
440.800045	10832.001154	30.383706
441.174759	10845.526460	30.388724
441.421778	10868.622984	30.393741
441.626505	10877.631185	30.398759
442.050788	10909.354782	30.403776
442.670456	10927.196167	30.408794
443.060992	10934.824070	30.413812
443.335230	10969.554943	30.418829
443.498944	10981.225021	30.423847
444.181538	11006.861989	30.428864
444.356956	11033.522039	30.433882
445.056234	11061.619329	30.438900
445.102575	11083.879049	30.443917
445.683875	11105.114577	30.448935
446.304626	11142.693575	30.453952
446.540352	11165.650136	30.458970
447.010987	11185.990463	30.463988
447.720433	11215.867243	30.469005
448.126962	11237.436410	30.474023
448.472326	11262.283168	30.479040
448.949506	11295.499013	30.484058
449.689616	11311.897967	30.489076
449.628332	11337.041790	30.494093
450.442204	11348.787704	30.499111
450.648552	11370.874451	30.504128
450.949028	11401.203574	30.509146
451.692076	11415.174003	30.514164
451.848082	11439.270559	30.519181
451.944122	11464.888955	30.524199
452.770348	11484.122779	30.529216
453.346140	11516.420600	30.534234
454.023533	11531.506488	30.539252
454.295164	11554.966307	30.544269
454.963977	11570.271435	30.549287
455.594061	11592.462986	30.554304
456.004662	11610.425986	30.559322
456.363244	11617.876003	30.564340
456.786600	11643.367905	30.569357
457.375428	11658.843438	30.574375
457.733959	11671.547729	30.579392
457.847802	11698.894039	30.584410
458.854151	11708.033611	30.589428
459.424816	11732.602784	30.594445
459.739149	11746.400225	30.599463
460.287459	11771.061342	30.604480
460.687144	11801.653539	30.609498
461.440927	11809.888352	30.614516
461.741962	11824.758355	30.619533
461.832507	11853.655755	30.624551
462.270735	11865.087875	30.629568
463.244947	11869.256102	30.634586
464.401968	11878.305992	30.639604
464.965772	11888.524991	30.644621
465.042102	11901.876481	30.649639
465.531734	11915.422564	30.654656
465.602505	11934.098725	30.659674
466.427975	11951.315415	30.664692
466.497306	11965.792162	30.669709
466.913390	11988.068021	30.674727
467.166987	12001.294097	30.679744
467.312839	12032.639818	30.684762
467.904733	12048.696207	30.689780
468.288424	12076.768371	30.694797
468.196447	12107.295513	30.699815
469.130529	12137.505086	30.704832
469.154687	12174.967468	30.709850
469.943971	12194.217249	30.714868
470.182683	12224.563635	30.719885
470.449672	12250.702772	30.724903
471.322859	12293.309728	30.729920
471.641725	12321.464976	30.734938
471.966104	12351.251946	30.739956
472.739244	12385.222550	30.744973
473.344694	12416.251059	30.749991
474.119067	12434.249791	30.755008
474.587117	12462.899894	30.760026
475.845836	12467.355528	30.765044
476.434453	12490.018787	30.770061
476.792176	12505.483633	30.775079
477.660693	12505.140261	30.780096
477.681028	12520.859739	30.785114
478.020016	12542.905112	30.790132
478.527923	12554.936252	30.795149
478.729411	12575.222099	30.800167
479.311862	12593.929780	30.805184
479.397973	12614.119951	30.810202
479.842388	12640.721462	30.815220
480.358790	12665.808706	30.820237
480.904047	12700.557432	30.825255
480.892298	12711.362254	30.830272
481.444046	12745.576389	30.835290
481.967079	12766.421836	30.840308
482.443200	12796.991124	30.845325
483.016699	12824.185410	30.850343
483.570236	12838.527449	30.855360
483.898744	12872.113431	30.860378
483.878223	12897.887711	30.865396
484.548948	12920.301871	30.870413
484.724187	12947.612017	30.875431
485.142132	12979.119055	30.880448
485.495831	13012.104535	30.885466
486.131142	13040.562114	30.890484
486.787399	13075.622666	30.895501
487.030642	13103.386653	30.900519
488.113306	13130.126331	30.905536
488.582162	13160.239452	30.910554
489.466910	13171.738645	30.915572
490.166935	13202.103209	30.920589
490.706000	13226.549785	30.925607
491.182653	13241.080942	30.930624
491.506448	13269.101051	30.935642
491.494277	13290.188291	30.940660
492.553657	13317.629750	30.945677
492.448333	13344.794676	30.950695
493.452763	13379.157382	30.955712
493.437395	13406.639971	30.960730
494.582326	13413.194603	30.965748
494.729696	13443.481382	30.970765
495.058529	13470.878900	30.975783
496.138157	13495.197460	30.980800
496.226834	13521.858752	30.985818
496.962341	13552.117304	30.990836
497.366082	13578.183307	30.995853
497.828927	13607.489650	31.000871
498.325938	13634.551747	31.005888
498.372745	13665.135591	31.010906
499.174083	13693.347253	31.015924
499.736199	13720.664605	31.020941
500.191728	13753.885006	31.025959
500.880172	13777.453236	31.030976
501.164015	13808.164624	31.035994
502.503174	13825.028323	31.041012
503.354551	13835.162564	31.046029
503.706763	13854.883152	31.051047
504.409826	13860.824613	31.056064
504.545992	13886.926381	31.061082
504.974468	13910.762623	31.066100
505.972526	13920.236165	31.071117
506.259488	13940.863866	31.076135
506.457778	13965.029703	31.081152
506.459532	13982.730187	31.086170
506.599061	14003.396698	31.091188
507.690175	14027.619418	31.096205
507.772214	14061.558523	31.101223
508.679300	14092.501780	31.106240
509.343816	14111.198192	31.111258
509.784314	14135.904457	31.116276
510.341238	14164.224348	31.121293
510.198948	14196.638557	31.126311
511.171396	14216.187173	31.131328
511.093364	14252.264258	31.136346
511.645625	14288.631727	31.141364
512.823728	14313.602360	31.146381
512.871822	14341.193270	31.151399
513.612039	14363.446740	31.156416
514.351209	14406.253026	31.161434
514.429586	14429.070683	31.166452
514.922075	14454.533519	31.171469
515.201378	14489.649061	31.176487
516.054578	14514.702120	31.181504
516.144148	14550.756837	31.186522
516.852516	14566.348795	31.191540
517.504555	14594.177650	31.196557
517.600135	14631.087426	31.201575
518.046342	14659.864268	31.206592
518.614119	14685.839939	31.211610
519.472250	14712.222053	31.216628
520.202519	14742.833874	31.221645
520.182010	14766.434751	31.226663
521.028213	14791.362940	31.231680
521.458352	14822.248997	31.236698
522.352019	14865.565990	31.241716
522.972310	14881.819337	31.246733
522.880699	14917.151316	31.251751
523.320087	14940.276571	31.256768
524.079738	14975.245592	31.261786
524.514096	14997.705330	31.266804
525.055026	15030.633595	31.271821
525.234981	15069.192276	31.276839
525.934681	15106.909003	31.281856
526.563053	15141.788231	31.286874
526.880933	15175.323099	31.291892
527.838181	15203.550637	31.296909
528.301914	15243.676170	31.301927
529.124762	15267.316919	31.306944
529.714549	15301.273935	31.311962
529.928189	15335.564333	31.316980
530.665919	15359.490053	31.321997
531.229554	15388.246557	31.327015
531.572436	15419.005045	31.332032
532.586823	15452.750953	31.337050
532.827760	15484.387613	31.342068
533.807279	15500.323433	31.347085
534.042150	15546.672222	31.352103
534.717108	15557.965508	31.357120
535.513340	15584.674296	31.362138
535.984685	15615.624705	31.367156
536.503764	15640.383856	31.372173
536.850566	15674.909952	31.377191
537.333084	15700.688677	31.382208
537.883045	15725.499979	31.387226
538.262788	15749.519819	31.392244
538.809178	15776.327776	31.397261
539.214927	15809.287905	31.402279
539.836975	15844.456807	31.407296
540.451076	15874.491614	31.412314
540.579497	15908.843681	31.417332
541.448184	15941.779344	31.422349
541.768648	15983.072042	31.427367
542.572266	16016.529612	31.432384
543.051547	16039.798431	31.437402
543.485592	16078.853350	31.442420
544.365090	16103.500142	31.447437
544.878951	16141.317328	31.452455
545.521324	16166.778070	31.457472
546.069061	16194.796052	31.462490
546.528325	16238.370132	31.467508
547.694015	16253.396420	31.472525
547.937170	16272.912247	31.477543
548.517178	16308.085388	31.482560
549.043131	16326.034910	31.487578
549.381733	16361.984790	31.492596
550.067105	16389.902672	31.497613
550.675253	16415.596477	31.502631
550.777984	16445.970777	31.507648
551.684426	16469.593687	31.512666
552.034625	16497.813418	31.517684
552.447891	16538.976006	31.522701
552.908203	16568.467330	31.527719
553.371412	16590.877074	31.532736
553.400378	16625.842848	31.537754
553.856541	16652.473415	31.542772
554.764897	16688.609994	31.547789
555.083480	16728.991803	31.552807
555.661336	16756.923799	31.557824
556.198539	16797.483334	31.562842
556.902027	16829.138643	31.567860
557.556758	16865.592982	31.572877
557.731080	16899.601721	31.577895
558.614998	16937.432353	31.582912
558.990380	16964.246486	31.587930
559.661489	17015.180192	31.592948
560.561078	17043.147798	31.597965
560.769388	17084.308716	31.602983
561.560900	17110.372877	31.608000
562.514373	17149.500720	31.613018
562.545043	17179.773690	31.618036
563.293081	17213.384135	31.623053
563.555526	17249.306469	31.628071
564.472849	17288.206491	31.633088
565.052305	17320.292527	31.638106
565.377432	17359.641798	31.643124
566.007094	17385.333552	31.648141
566.634928	17437.870180	31.653159
567.370589	17472.654829	31.658176
567.932949	17503.748885	31.663194
568.623114	17533.806035	31.668212
569.476227	17566.806928	31.673229
569.951061	17601.250226	31.678247
570.739696	17632.283996	31.683264
571.377269	17652.924293	31.688282
571.912857	17696.372926	31.693300
572.647399	17718.413251	31.698317
572.934068	17750.990947	31.703335
573.308628	17790.668214	31.708352
574.191428	17818.857507	31.713370
574.646102	17861.447329	31.718388
574.821307	17885.994427	31.723405
575.446214	17919.113574	31.728423
575.763468	17963.512801	31.733440
576.674510	18005.216965	31.738458
577.019135	18043.389576	31.743476
577.424364	18071.975768	31.748493
578.198493	18120.063037	31.753511
578.578242	18154.534758	31.758528
579.551958	18194.991375	31.763546
579.952782	18241.412420	31.768564
580.546327	18270.746626	31.773581
581.100779	18314.301107	31.778599
581.924858	18358.255930	31.783616
582.868701	18384.648720	31.788634
582.933420	18426.687701	31.793652
583.785276	18462.331010	31.798669
584.202526	18496.955439	31.803687
584.829021	18535.116727	31.808704
586.082421	18554.215420	31.813722
586.456651	18589.023600	31.818740
587.194329	18622.935035	31.823757
587.664444	18650.589625	31.828775
588.469053	18676.871822	31.833792
589.405559	18690.094151	31.838810
589.941531	18729.015381	31.843828
590.282276	18752.672305	31.848845
590.996222	18769.246046	31.853863
590.977025	18794.506854	31.858880
591.974272	18818.080610	31.863898
592.644211	18853.557116	31.868916
593.195367	18875.437783	31.873933
593.272852	18902.686354	31.878951
593.561422	18931.096129	31.883968
594.131309	18955.020874	31.888986
594.462256	18987.126252	31.894004
595.408628	19016.311899	31.899021
595.931903	19051.034529	31.904039
596.553372	19092.457598	31.909056
597.575360	19111.258034	31.914074
597.523687	19151.238192	31.919092
598.511756	19178.636009	31.924109
598.764873	19216.142864	31.929127
599.562219	19250.602066	31.934144
600.418954	19293.378834	31.939162
600.609759	19326.706956	31.944180
601.274867	19354.730211	31.949197
602.014276	19393.450524	31.954215
602.104937	19432.998449	31.959232
603.250184	19468.111468	31.964250
603.739408	19507.862845	31.969268
604.826229	19541.772077	31.974285
605.137413	19575.656805	31.979303
605.727714	19610.774340	31.984320
606.359525	19635.012491	31.989338
607.038157	19674.671546	31.994356
607.626094	19708.090125	31.999373
608.311050	19741.120905	32.004391
608.320193	19790.854007	32.009408
609.093006	19819.928887	32.014426
609.803120	19872.642522	32.019444
610.187802	19904.677870	32.024461
611.202176	19940.570265	32.029479
611.568340	19988.176010	32.034496
613.549989	20008.028333	32.039514
614.252803	20043.173358	32.044532
614.521289	20068.018271	32.049549
615.185498	20083.337286	32.054567
615.481222	20112.967040	32.059584
616.297753	20142.686349	32.064602
617.155654	20167.825031	32.069620
617.159885	20203.338133	32.074637
618.025218	20230.794449	32.079655
618.438876	20268.461558	32.084672
618.700808	20301.704456	32.089690
619.295405	20335.615881	32.094708
619.908881	20376.430074	32.099725
620.301735	20423.937954	32.104743
620.772740	20460.711974	32.109760
621.825109	20502.311048	32.114778
622.265477	20551.416641	32.119796
622.431346	20593.438228	32.124813
623.518573	20620.734187	32.129831
623.823920	20667.643421	32.134848
624.688695	20710.017683	32.139866
624.757018	20770.649233	32.144884
625.664994	20813.800451	32.149901
626.423452	20853.689564	32.154919
626.977199	20899.783542	32.159936
627.522675	20942.669245	32.164954
628.197830	20993.300002	32.169972
628.673195	21048.447972	32.174989
629.443571	21080.842208	32.180007
629.994754	21135.517385	32.185024
631.109571	21170.417066	32.190042
631.715582	21209.490298	32.195060
632.621602	21249.748983	32.200077
633.402630	21280.625488	32.205095
633.871811	21316.820108	32.210112
634.500746	21336.688507	32.215130
635.114897	21374.535036	32.220148
635.939486	21400.331283	32.225165
636.687850	21429.140674	32.230183
637.266195	21463.031306	32.235200
638.141823	21485.110810	32.240218
638.651482	21515.954109	32.245236
638.980729	21537.442656	32.250253
639.696485	21574.806188	32.255271
640.060585	21610.764970	32.260288
640.277672	21644.863797	32.265306
640.905997	21686.607219	32.270324
641.546039	21730.686752	32.275341
642.410732	21775.963523	32.280359
642.639396	21822.558886	32.285376
643.578314	21860.684356	32.290394
644.318839	21897.930913	32.295412
644.793886	21946.497515	32.300429
645.453236	21993.215792	32.305447
646.070699	22032.667992	32.310464
646.764001	22061.739625	32.315482
647.675001	22108.071476	32.320500
648.385867	22151.414283	32.325517
649.003925	22183.682403	32.330535
649.819489	22230.225277	32.335552
650.419376	22267.494425	32.340570
651.477706	22306.088707	32.345588
651.737951	22341.508943	32.350605
652.758076	22376.216993	32.355623
653.056093	22419.845813	32.360640
653.733948	22460.104581	32.365658
654.365302	22498.456090	32.370676
654.720515	22547.523049	32.375693
655.894786	22574.605980	32.380711
656.170271	22618.213470	32.385728
657.036781	22667.719273	32.390746
657.741931	22706.242942	32.395764
658.109233	22755.624476	32.400781
658.522640	22790.964804	32.405799
659.270390	22846.517718	32.410816
660.216469	22889.383207	32.415834
661.186750	22936.251196	32.420852
661.462312	22982.728251	32.425869
662.161952	23020.280278	32.430887
662.623208	23075.903709	32.435904
663.004146	23103.616381	32.440922
663.970343	23160.399956	32.445940
664.742300	23205.808182	32.450957
665.434920	23248.833967	32.455975
665.732641	23304.262331	32.460992
666.864008	23349.855059	32.466010
667.077693	23396.835598	32.471028
667.957060	23440.913282	32.476045
669.126944	23487.669355	32.481063
669.640580	23529.194397	32.486080
670.563491	23578.124978	32.491098
671.263390	23605.776059	32.496116
671.592209	23647.563925	32.501133
672.580591	23696.143372	32.506151
672.939029	23740.119560	32.511168
673.515907	23787.044481	32.516186
674.133288	23819.972566	32.521204
674.774171	23874.622393	32.526221
675.503488	23918.206322	32.531239
676.544504	23968.509702	32.536256
677.194118	24000.561016	32.541274
678.607648	24020.164638	32.546292
679.254131	24055.483570	32.551309
679.821237	24084.622055	32.556327
680.539846	24115.727565	32.561344
680.934721	24139.262480	32.566362
681.848474	24161.945696	32.571380
682.096868	24201.396473	32.576397
682.715783	24230.021562	32.581415
683.296788	24272.618267	32.586432
683.485158	24310.561969	32.591450
684.333324	24350.185085	32.596468
684.885623	24396.508612	32.601485
685.534683	24431.012614	32.606503
685.813092	24475.306210	32.611520
686.621025	24523.252232	32.616538
687.155667	24573.977216	32.621556
687.379228	24626.596025	32.626573
688.499332	24668.768405	32.631591
689.379541	24717.803224	32.636608
690.098372	24778.604860	32.641626
690.907006	24823.037867	32.646644
691.489740	24869.528379	32.651661
692.518672	24920.979872	32.656679
692.974651	24975.282326	32.661696
693.709958	25022.059098	32.666714
694.745624	25068.656511	32.671732
694.636353	25120.273062	32.676749
695.540715	25170.031982	32.681767
696.174628	25226.310727	32.686784
696.889268	25281.799750	32.691802
697.996574	25323.476253	32.696820
698.758370	25394.207548	32.701837
699.538107	25429.495527	32.706855
700.638421	25485.184181	32.711872
701.108358	25531.371482	32.716890
702.059581	25578.539361	32.721908
702.319256	25622.547700	32.726925
702.891591	25669.717897	32.731943
703.733077	25719.007666	32.736960
704.356588	25764.356345	32.741978
705.663554	25816.196601	32.746996
705.927947	25861.948993	32.752013
707.069290	25899.665194	32.757031
708.041284	25949.169045	32.762048
708.978043	25988.389783	32.767066
709.529805	26025.622894	32.772084
710.261684	26078.956362	32.777101
711.066904	26108.907591	32.782119
711.364273	26150.155744	32.787136
711.855192	26204.696236	32.792154
712.583667	26242.085516	32.797172
713.382322	26294.638128	32.802189
714.027695	26337.140719	32.807207
714.282200	26395.390427	32.812224
715.409632	26444.270901	32.817242
716.235447	26493.223727	32.822260
716.374611	26543.724527	32.827277
717.648488	26589.732226	32.832295
718.094194	26633.770693	32.837312
718.429782	26692.261436	32.842330
719.293213	26743.338877	32.847348
719.900677	26815.300004	32.852365
720.520453	26863.072338	32.857383
721.192926	26915.437645	32.862400
721.945683	26975.223095	32.867418
722.960389	27027.958869	32.872436
723.894472	27079.550735	32.877453
724.737561	27120.665355	32.882471
725.871750	27166.468587	32.887488
726.647828	27212.302389	32.892506
727.161377	27252.166608	32.897524
727.662824	27299.054597	32.902541
728.369838	27331.797525	32.907559
729.204080	27375.176697	32.912576
730.192971	27412.597129	32.917594
730.614104	27438.388166	32.922612
731.147357	27493.001385	32.927629
731.833558	27537.320396	32.932647
732.720253	27580.660241	32.937664
733.370336	27632.778074	32.942682
733.788589	27676.374336	32.947700
734.381751	27714.735461	32.952717
735.052110	27777.443485	32.957735
735.970333	27816.620097	32.962752
736.909467	27873.275857	32.967770
738.489369	27912.039949	32.972788
739.109293	27953.190999	32.977805
739.844427	27988.642090	32.982823
740.806604	28021.592910	32.987840
741.442426	28061.041494	32.992858
742.419055	28102.914740	32.997876
743.156517	28144.047880	33.002893
743.204641	28183.752521	33.007911
743.557495	28226.279331	33.012928
744.451038	28280.522553	33.017946
745.602980	28316.402336	33.022964
746.058743	28379.132979	33.027981
746.844683	28429.898060	33.032999
747.694604	28481.614044	33.038016
748.036852	28527.752212	33.043034
748.846464	28578.457093	33.048052
749.607393	28636.729204	33.053069
750.546717	28684.974377	33.058087
751.179189	28735.056191	33.063104
751.485681	28790.416110	33.068122
752.283368	28845.661790	33.073140
752.832416	28912.639729	33.078157
753.615101	28961.377675	33.083175
754.622125	29027.665262	33.088192
755.129517	29097.614745	33.093210
756.072319	29147.124631	33.098228
756.967105	29208.025964	33.103245
758.344154	29260.502536	33.108263
758.966856	29300.524437	33.113280
759.641820	29359.785407	33.118298
760.915768	29411.380849	33.123316
762.145151	29460.594047	33.128333
762.367436	29497.050451	33.133351
763.413044	29540.837479	33.138368
764.226458	29591.803441	33.143386
765.104561	29628.562531	33.148404
765.766366	29685.822741	33.153421
766.504612	29726.427983	33.158439
766.728705	29767.871864	33.163456
767.529031	29822.266431	33.168474
768.249071	29876.092103	33.173492
768.898730	29931.882084	33.178509
769.629893	29978.942746	33.183527
770.305380	30040.670826	33.188544
770.696585	30095.983154	33.193562
772.057022	30145.354588	33.198580
772.872001	30202.288978	33.203597
773.424114	30258.961030	33.208615
774.448548	30308.688578	33.213632
774.840787	30358.944500	33.218650
775.875168	30405.124537	33.223668
776.711552	30473.858067	33.228685
777.368503	30521.140122	33.233703
778.063871	30569.377138	33.238720
778.566166	30623.004773	33.243738
779.194989	30660.803279	33.248756
780.037207	30723.487252	33.253773
780.860712	30771.603653	33.258791
781.269584	30821.712723	33.263808
782.054832	30877.161769	33.268826
783.047055	30931.668465	33.273844
784.008870	30973.511964	33.278861
784.771176	31034.900793	33.283879
785.791852	31086.249085	33.288896
786.345921	31145.104158	33.293914
786.947734	31201.303274	33.298932
787.974483	31256.861139	33.303949
788.388552	31306.490141	33.308967
789.869430	31360.631114	33.313984
790.593409	31413.625747	33.319002
791.563670	31461.859986	33.324020
792.941101	31503.323783	33.329037
793.799331	31552.587122	33.334055
794.614930	31595.573560	33.339072
795.067998	31648.895439	33.344090
795.790777	31691.864917	33.349108
796.504798	31742.472373	33.354125
797.206758	31786.690650	33.359143
798.315428	31834.961107	33.364160
798.760259	31889.302673	33.369178
799.417382	31941.550463	33.374196
800.739431	32000.623467	33.379213
801.042593	32055.935777	33.384231
801.670940	32107.297100	33.389248
802.620967	32180.639801	33.394266
803.152417	32227.237254	33.399284
803.922429	32284.974601	33.404301
804.719766	32350.818738	33.409319
805.713843	32409.589938	33.414336
806.263815	32473.747111	33.419354
806.982507	32534.432799	33.424372
808.147504	32592.659517	33.429389
808.912067	32660.045952	33.434407
809.528547	32711.985908	33.439424
810.339086	32793.596268	33.444442
810.649988	32845.925511	33.449460
812.191950	32915.353867	33.454477
812.470527	32976.463383	33.459495
814.204165	33044.256543	33.464512
814.892120	33110.170682	33.469530
815.736226	33159.509569	33.474548
816.889806	33215.318455	33.479565
817.708078	33271.641199	33.484583
819.100584	33314.705760	33.489600
819.552223	33378.741934	33.494618
820.355797	33419.350572	33.499636
821.326447	33467.538826	33.504653
821.657043	33520.922491	33.509671
822.928250	33574.526558	33.514688
823.488880	33630.795542	33.519706
824.305394	33682.093517	33.524724
825.444788	33733.278135	33.529741
825.974125	33799.276035	33.534759
826.695031	33847.516685	33.539776
827.465655	33902.931817	33.544794
828.214224	33964.634893	33.549812
828.773969	34017.547912	33.554829
829.491701	34084.193868	33.559847
830.586394	34125.112608	33.564864
831.223621	34200.610110	33.569882
832.231838	34257.601397	33.574900
832.931091	34307.926541	33.579917
833.479685	34358.237324	33.584935
834.479116	34405.310508	33.589952
835.039643	34472.601766	33.594970
835.427166	34525.239393	33.599988
836.716996	34582.617652	33.605005
837.437884	34646.451393	33.610023
838.393386	34707.485863	33.615040
839.017868	34768.546749	33.620058
840.276212	34815.865063	33.625076
841.496512	34864.485533	33.630093
842.630724	34921.509586	33.635111
843.717797	34967.931806	33.640128
844.419305	35024.150976	33.645146
845.320812	35069.002682	33.650164
846.255521	35113.236020	33.655181
846.819845	35166.555862	33.660199
847.660550	35208.793427	33.665216
848.406978	35269.779877	33.670234
848.704193	35331.987162	33.675252
849.914392	35380.281613	33.680269
850.728266	35439.664727	33.685287
851.364694	35504.431008	33.690304
852.365421	35569.735119	33.695322
852.996933	35624.569447	33.700340
854.068192	35688.117853	33.705357
854.765634	35755.986230	33.710375
856.054118	35816.314497	33.715392
856.803671	35882.727235	33.720410
857.487762	35932.603366	33.725428
858.360323	36002.367430	33.730445
859.067053	36065.018950	33.735463
860.061569	36121.328205	33.740480
861.197075	36189.313142	33.745498
862.208279	36250.963048	33.750516
862.822580	36298.580953	33.755533
863.477543	36369.783801	33.760551
864.564207	36429.297944	33.765568
865.818706	36482.058401	33.770586
866.481852	36555.834080	33.775604
867.554220	36608.288079	33.780621
868.264344	36665.509309	33.785639
868.966671	36718.982294	33.790656
869.816773	36773.576899	33.795674
870.977579	36846.112658	33.800692
871.931513	36900.729365	33.805709
872.260675	36972.212577	33.810727
873.165704	37030.922015	33.815744
874.117793	37094.840955	33.820762
875.262170	37158.578397	33.825780
876.641072	37203.455155	33.830797
877.935377	37261.465982	33.835815
878.588886	37306.873211	33.840832
879.605360	37359.027918	33.845850
880.540347	37407.338209	33.850868
881.186523	37457.539981	33.855885
882.000931	37512.685841	33.860903
883.076698	37559.804741	33.865920
883.763857	37620.933627	33.870938
884.557192	37673.958525	33.875956
885.561293	37719.103383	33.880973
886.483481	37776.300903	33.885991
886.941334	37828.670182	33.891008
888.073202	37888.339447	33.896026
888.609782	37938.919846	33.901044
889.792210	37997.247290	33.906061
890.388082	38060.402513	33.911079
891.410239	38110.344936	33.916096
891.885324	38172.564437	33.921114
892.565653	38222.908128	33.926132
893.622839	38275.058731	33.931149
894.295073	38329.994853	33.936167
895.041573	38388.625192	33.941184
896.308620	38450.228976	33.946202
896.754423	38504.815050	33.951220
898.124866	38563.905224	33.956237
898.706989	38622.359432	33.961255
899.421493	38691.695252	33.966272
900.011826	38747.498889	33.971290
900.787975	38826.861293	33.976308
902.172426	38878.203567	33.981325
902.676592	38954.130710	33.986343
903.810607	39018.722683	33.991360
905.056432	39090.633075	33.996378
905.706273	39153.454264	34.001396
906.523108	39221.586977	34.006413
907.477068	39291.557780	34.011431
908.018072	39361.352783	34.016448
908.947949	39435.640700	34.021466
909.910905	39515.166272	34.026484
911.073778	39581.475549	34.031501
911.794662	39666.958591	34.036519
912.868766	39723.758199	34.041536
913.817318	39809.769201	34.046554
914.996874	39887.915407	34.051572
915.995984	39943.361270	34.056589
917.072284	40016.458435	34.061607
917.998046	40087.024339	34.066624
919.115570	40152.526615	34.071642
919.971116	40219.903872	34.076660
921.197244	40282.391988	34.081677
922.086218	40353.894138	34.086695
922.564870	40421.178907	34.091712
924.011461	40481.445103	34.096730
924.388753	40551.908166	34.101748
925.844052	40613.710165	34.106765
926.553479	40688.675441	34.111783
927.348292	40755.444031	34.116800
928.722673	40809.676344	34.121818
929.353479	40884.496423	34.126836
930.169613	40948.213953	34.131853
931.442977	41021.302795	34.136871
932.377172	41084.173851	34.141888
933.890765	41143.482793	34.146906
934.399160	41210.695800	34.151924
935.536184	41266.205788	34.156941
936.338191	41335.865311	34.161959
937.004805	41403.206069	34.166976
937.875744	41464.475321	34.171994
938.478444	41537.075784	34.177012
939.941983	41601.105538	34.182029
940.699748	41669.824328	34.187047
941.637876	41743.416816	34.192064
942.710804	41805.484103	34.197082
943.442366	41877.167540	34.202100
944.269636	41945.402029	34.207117
945.097726	42026.627474	34.212135
945.832363	42088.311819	34.217152
947.116965	42155.906551	34.222170
947.959471	42239.723671	34.227188
949.354060	42303.728266	34.232205
950.137504	42366.759292	34.237223
950.992093	42446.653964	34.242240
951.980216	42511.974746	34.247258
952.908106	42593.249999	34.252276
953.885374	42651.482746	34.257293
955.044713	42706.037858	34.262311
955.783635	42774.282349	34.267328
956.577024	42825.219962	34.272346
957.368515	42882.539829	34.277364
958.294658	42941.122847	34.282381
959.281544	43007.703955	34.287399
960.240005	43077.806373	34.292416
960.872928	43134.411556	34.297434
962.256892	43209.957226	34.302452
963.543666	43279.022476	34.307469
964.412942	43336.116364	34.312487
965.417041	43400.596062	34.317504
966.304819	43466.732252	34.322522
967.192281	43533.077418	34.327540
968.238186	43590.973058	34.332557
969.249530	43658.210133	34.337575
969.854265	43735.978845	34.342592
970.855706	43798.088181	34.347610
971.776977	43876.440631	34.352628
973.096252	43943.434558	34.357645
974.451564	44015.805858	34.362663
975.141300	44078.470520	34.367680
976.278205	44143.304900	34.372698
976.741831	44216.403906	34.377716
978.013027	44275.518676	34.382733
979.053671	44348.787637	34.387751
979.756977	44428.656094	34.392768
980.709620	44498.985306	34.397786
981.649950	44578.033057	34.402804
982.336667	44655.823855	34.407821
983.346671	44733.634181	34.412839
984.013875	44817.336546	34.417856
985.269556	44896.393269	34.422874
986.707446	44978.445505	34.427892
987.802082	45061.702723	34.432909
988.860456	45131.884639	34.437927
989.768259	45205.512351	34.442944
990.891488	45265.607949	34.447962
992.101553	45352.093312	34.452980
992.898458	45426.415857	34.457997
994.231363	45491.394447	34.463015
995.724028	45574.167800	34.468032
996.277017	45636.858130	34.473050
997.482121	45699.345916	34.478068
998.602510	45779.407312	34.483085
999.375877	45847.510392	34.488103
1000.130889	45921.354017	34.493120
1001.076030	45998.717065	34.498138
1002.408583	46068.814962	34.503156
1003.374827	46131.530910	34.508173
1004.349840	46203.823019	34.513191
1004.970219	46281.939765	34.518208
1006.042484	46353.356897	34.523226
1007.183034	46422.884828	34.528244
1008.083679	46505.412174	34.533261
1009.263410	46581.791822	34.538279
1010.005273	46654.045759	34.543296
1011.311895	46721.486491	34.548314
1012.312621	46797.508849	34.553332
1013.209564	46867.265854	34.558349
1014.607083	46938.830323	34.563367
1015.135050	47020.266223	34.568384
1016.212234	47093.146263	34.573402
1017.061874	47166.327655	34.578420
1018.028717	47241.331950	34.583437
1019.281045	47319.366576	34.588455
1019.761908	47393.921953	34.593472
1021.157064	47465.146846	34.598490
1022.209646	47543.839634	34.603508
1023.047869	47594.730549	34.608525
1024.313685	47662.635938	34.613543
1025.080915	47735.047542	34.618560
1026.149977	47800.187751	34.623578
1027.416721	47867.568527	34.628596
1028.655497	47923.345018	34.633613
1030.016516	47987.238315	34.638631
1030.734973	48058.273071	34.643648
1031.572150	48109.177958	34.648666
1032.359334	48177.456735	34.653684
1033.487494	48244.107360	34.658701
1034.680658	48308.565437	34.663719
1035.284920	48383.402202	34.668736
1036.379863	48451.545327	34.673754
1036.799648	48536.894304	34.678772
1038.403586	48609.501108	34.683789
1039.460365	48685.154141	34.688807
1040.232787	48771.834623	34.693824
1041.327652	48858.693000	34.698842
1042.315314	48932.326774	34.703860
1043.509930	49020.239438	34.708877
1044.714151	49099.717497	34.713895
1045.541487	49177.742420	34.718912
1046.547163	49270.474763	34.723930
1047.930742	49348.888189	34.728948
1048.760380	49432.664628	34.733965
1049.762789	49512.169209	34.738983
1051.020633	49604.977538	34.744000
1052.070016	49681.792830	34.749018
1053.519855	49755.148528	34.754036
1054.323875	49844.162763	34.759053
1055.662393	49918.991495	34.764071
1056.424333	50011.707837	34.769088
1057.798323	50089.644448	34.774106
1058.989887	50167.502162	34.779124
1059.742553	50247.807404	34.784141
1060.998325	50322.080903	34.789159
1062.016191	50404.370052	34.794176
1063.017843	50485.959718	34.799194
1064.237664	50571.065201	34.804212
1065.244311	50648.282657	34.809229
1066.434875	50718.765004	34.814247
1067.565473	50806.764083	34.819264
1068.493889	50876.503152	34.824282
1069.658995	50961.789429	34.829300
1070.721001	51035.083040	34.834317
1071.890233	51123.766979	34.839335
1072.952195	51205.349803	34.844352
1074.227751	51278.104766	34.849370
1075.282581	51348.154601	34.854388
1076.198616	51433.690190	34.859405
1077.141193	51511.774695	34.864423
1078.222152	51593.729244	34.869440
1079.507481	51671.109217	34.874458
1080.509144	51751.140491	34.879476
1081.378187	51836.881032	34.884493
1082.577210	51917.761671	34.889511
1083.441340	51993.980761	34.894528
1084.307695	52070.921088	34.899546
1085.926085	52165.341403	34.904564
1087.017850	52240.848827	34.909581
1087.781772	52319.957283	34.914599
1088.918996	52414.326955	34.919616
1090.170236	52486.425101	34.924634
1091.419649	52559.181826	34.929652
1092.561094	52636.973400	34.934669
1093.721694	52717.793199	34.939687
1094.631764	52787.028331	34.944704
1095.535618	52863.971770	34.949722
1096.975024	52926.132816	34.954740
1097.691974	53004.997800	34.959757
1099.208874	53062.863272	34.964775
1100.393923	53121.122241	34.969792
1101.256737	53194.535937	34.974810
1102.530649	53259.760970	34.979828
1103.095556	53333.683404	34.984845
1104.525406	53404.737808	34.989863
1105.542251	53478.343565	34.994880
1106.403700	53558.409200	34.999898
1107.752256	53623.788155	35.004916
1108.263214	53705.338954	35.009933
1109.440352	53772.213085	35.014951
1110.342790	53871.497706	35.019968
1111.695797	53962.467235	35.024986
1112.615228	54039.412113	35.030004
1113.797348	54129.092660	35.035021
1115.077246	54216.518196	35.040039
1116.103983	54313.070595	35.045056
1117.047849	54394.138744	35.050074
1118.053003	54475.330522	35.055092
1118.928917	54569.629322	35.060109
1119.850950	54662.535448	35.065127
1121.212021	54760.328587	35.070144
1122.542938	54857.316811	35.075162
1123.905601	54954.116973	35.080180
1124.829598	55049.169594	35.085197
1126.121620	55130.148109	35.090215
1127.581653	55231.585556	35.095232
1128.687313	55312.498779	35.100250
1130.217819	55405.199202	35.105268
1131.123044	55499.971778	35.110285
1132.250002	55583.964547	35.115303
1133.448238	55686.431927	35.120320
1134.518864	55766.871192	35.125338
1135.870454	55863.170516	35.130356
1137.192823	55949.906047	35.135373
1138.062265	56035.370743	35.140391
1138.991203	56136.179601	35.145408
1139.788796	56226.295012	35.150426
1141.587349	56311.356605	35.155444
1142.214284	56409.998614	35.160461
1143.433404	56497.948328	35.165479
1145.021427	56593.821429	35.170496
1145.936459	56685.053130	35.175514
1147.584969	56776.677309	35.180532
1148.527988	56865.348529	35.185549
1149.739519	56949.611418	35.190567
1151.082791	57042.094213	35.195584
1151.884460	57140.091813	35.200602
1153.166878	57226.863523	35.205620
1154.532291	57312.141670	35.210637
1155.463609	57396.297855	35.215655
1156.595950	57491.770818	35.220672
1157.646816	57585.294867	35.225690
1159.260015	57674.541965	35.230708
1160.703492	57762.663934	35.235725
1161.648022	57838.971651	35.240743
1162.902506	57921.889519	35.245760
1163.883126	58013.881883	35.250778
1165.030032	58092.810785	35.255796
1166.228417	58177.307881	35.260813
1167.420511	58260.622704	35.265831
1168.459536	58351.252831	35.270848
1169.332226	58445.580115	35.275866
1170.667171	58521.835555	35.280884
1171.637689	58600.521419	35.285901
1172.978945	58676.244710	35.290919
1174.027818	58753.266944	35.295936
1174.824498	58834.309798	35.300954
1176.170429	58909.767263	35.305972
1176.959439	59003.584418	35.310989
1178.337653	59090.727696	35.316007
1179.524595	59169.426030	35.321024
1180.530358	59261.685066	35.326042
1181.833399	59339.891178	35.331060
1182.542737	59435.488311	35.336077
1184.024005	59517.281365	35.341095
1185.146218	59619.998900	35.346112
1186.112131	59719.240976	35.351130
1187.932240	59802.102571	35.356148
1188.877384	59894.246854	35.361165
1190.164395	59979.647903	35.366183
1191.277879	60083.102984	35.371200
1192.245416	60174.421992	35.376218
1193.815714	60271.236607	35.381236
1194.772467	60357.880363	35.386253
1196.346583	60447.099467	35.391271
1197.964388	60536.824804	35.396288
1199.424636	60609.642920	35.401306
1201.267178	60681.908026	35.406324
1202.635467	60772.021203	35.411341
1203.642068	60848.638889	35.416359
1205.242351	60915.384824	35.421376
1206.249832	61000.174652	35.426394
1207.354192	61075.119410	35.431412
1208.360988	61154.839658	35.436429
1209.317960	61239.467268	35.441447
1210.650790	61324.378483	35.446464
1211.277952	61419.591057	35.451482
1212.915568	61497.935579	35.456500
1213.762864	61579.289845	35.461517
1215.039329	61674.484628	35.466535
1216.440633	61770.692147	35.471552
1217.104454	61874.889440	35.476570
1218.551751	61959.253304	35.481588
1219.749961	62059.411890	35.486605
1221.089675	62151.807091	35.491623
1221.956890	62253.695473	35.496640
1223.390494	62354.749152	35.501658
1224.428660	62443.831049	35.506676
1225.747870	62543.270109	35.511693
1226.883593	62638.845014	35.516711
1228.191807	62738.343541	35.521728
1229.432377	62837.897309	35.526746
1230.735903	62924.837967	35.531764
1232.263536	63021.461155	35.536781
1233.697076	63112.458990	35.541799
1235.321957	63194.685079	35.546816
1235.934925	63297.775792	35.551834
1237.449777	63375.676930	35.556852
1238.850709	63475.537478	35.561869
1240.084948	63573.246679	35.566887
1241.338829	63658.823915	35.571904
1242.136091	63749.606593	35.576922
1243.604671	63841.316993	35.581940
1244.721257	63926.701280	35.586957
1245.766419	64034.330108	35.591975
1247.224302	64122.073906	35.596992
1248.188195	64224.696004	35.602010
1249.676524	64317.063468	35.607028
1250.485861	64417.368057	35.612045
1251.510860	64518.861312	35.617063
1253.353809	64604.653974	35.622080
1254.746394	64686.547628	35.627098
1256.091601	64767.581603	35.632116
1257.257017	64844.193254	35.637133
1258.046733	64928.232723	35.642151
1259.144847	65015.402566	35.647168
1260.325793	65103.642400	35.652186
1261.978080	65176.304777	35.657204
1263.122227	65270.970470	35.662221
1263.634792	65363.955827	35.667239
1265.286882	65460.765337	35.672256
1266.179909	65550.210122	35.677274
1267.470439	65652.008496	35.682292
1268.685024	65754.927036	35.687309
1269.662766	65856.350740	35.692327
1271.054626	65960.610038	35.697344
1272.271551	66078.281012	35.702362
1273.678172	66178.904842	35.707380
1275.227418	66297.607737	35.712397
1276.222776	66400.487052	35.717415
1277.552560	66501.466009	35.722432
1278.771049	66616.954962	35.727450
1280.311853	66724.619438	35.732468
1281.932034	66827.365241	35.737485
1282.812613	66949.619504	35.742503
1284.183874	67053.905497	35.747520
1285.569488	67159.234366	35.752538
1287.164524	67268.842777	35.757556
1288.370994	67381.779174	35.762573
1289.825329	67490.188465	35.767591
1291.295508	67591.922337	35.772608
1292.539718	67697.509704	35.777626
1294.192517	67796.841641	35.782644
1295.130316	67892.239370	35.787661
1296.351196	68007.480986	35.792679
1298.324222	68117.059529	35.797696
1299.342430	68213.262720	35.802714
1300.980181	68304.887004	35.807732
1302.511538	68401.637866	35.812749
1303.710174	68511.477928	35.817767
1305.012060	68602.706000	35.822784
1306.496282	68706.746874	35.827802
1307.731344	68800.664395	35.832820
1309.374662	68898.533096	35.837837
1310.423684	68997.001220	35.842855
1312.046283	69080.335896	35.847872
1313.069567	69187.648057	35.852890
1314.173833	69270.899398	35.857908
1315.690179	69371.164128	35.862925
1317.051274	69480.305513	35.867943
1318.273304	69570.688292	35.872960
1319.864340	69672.031668	35.877978
1321.466981	69766.566685	35.882996
1322.411439	69854.948410	35.888013
1323.641062	69956.931705	35.893031
1325.482646	70044.230956	35.898048
1326.295789	70147.919844	35.903066
1327.503117	70241.536642	35.908084
1328.900957	70336.827482	35.913101
1329.940293	70442.812583	35.918119
1331.316511	70543.027671	35.923136
1332.844875	70648.399252	35.928154
1333.852282	70745.886332	35.933172
1334.856997	70850.922306	35.938189
1335.760387	70967.271362	35.943207
1337.640407	71071.450096	35.948224
1339.167866	71170.972826	35.953242
1340.413587	71276.314947	35.958260
1342.118050	71363.209362	35.963277
1343.816850	71452.409960	35.968295
1345.366546	71518.330569	35.973312
1346.435169	71594.800157	35.978330
1348.220022	71673.159561	35.983348
1349.665250	71745.087555	35.988365
1350.798167	71830.502016	35.993383
1351.849081	71902.365165	35.998400
1353.759107	71973.993470	36.003418
1354.644782	72054.837026	36.008436
1356.227138	72149.567485	36.013453
1357.011260	72239.584390	36.018471
1357.876141	72325.409472	36.023488
1359.277523	72425.691178	36.028506
1360.501276	72522.644575	36.033524
1361.788256	72621.602298	36.038541
1362.558709	72726.504924	36.043559
1364.187032	72825.980231	36.048576
1365.978414	72942.035162	36.053594
1367.354211	73041.018628	36.058612
1368.666424	73130.551070	36.063629
1369.731910	73251.913288	36.068647
1371.588560	73351.329701	36.073664
1372.624779	73470.050316	36.078682
1373.983685	73573.167475	36.083700
1375.772494	73676.876751	36.088717
1377.088413	73790.146890	36.093735
1378.482898	73897.604218	36.098752
1379.919287	73994.124588	36.103770
1381.181579	74103.490575	36.108788
1382.636128	74220.198833	36.113805
1383.470583	74330.468313	36.118823
1385.083571	74440.705736	36.123840
1386.489645	74560.880937	36.128858
1387.807513	74676.434487	36.133876
1389.303084	74788.363590	36.138893
1390.593990	74919.945517	36.143911
1391.995878	75033.055547	36.148928
1393.484477	75150.801227	36.153946
1395.006956	75265.476801	36.158964
1396.420290	75384.210557	36.163981
1397.772972	75505.715647	36.168999
1399.023845	75625.223096	36.174016
1400.555561	75741.343287	36.179034
1401.965128	75868.553955	36.184052
1403.416666	75970.044552	36.189069
1404.594442	76096.570350	36.194087
1406.142102	76223.571189	36.199104
1407.985511	76344.991011	36.204122
1409.033903	76470.373309	36.209140
1410.588239	76578.057161	36.214157
1411.838193	76710.781592	36.219175
1413.092343	76827.367673	36.224192
1415.266041	76946.255959	36.229210
1416.341979	77058.880505	36.234228
1417.761666	77186.779835	36.239245
1419.195684	77307.596301	36.244263
1420.474814	77425.194470	36.249280
1422.286453	77540.582074	36.254298
1423.318628	77657.598961	36.259316
1425.168402	77773.513664	36.264333
1426.280014	77889.062369	36.269351
1427.933409	78012.330727	36.274368
1429.491766	78127.798238	36.279386
1430.630321	78242.976869	36.284404
1432.307445	78356.805341	36.289421
1434.147562	78458.143392	36.294439
1435.816878	78560.914579	36.299456
1437.189418	78665.252540	36.304474
1438.419955	78768.168807	36.309492
1439.907382	78858.795132	36.314509
1441.277072	78953.367298	36.319527
1442.327936	79038.817432	36.324544
1444.045322	79130.967084	36.329562
1445.003595	79242.516759	36.334580
1446.622126	79338.381715	36.339597
1447.827087	79450.311896	36.344615
1448.946175	79549.878562	36.349632
1450.576476	79667.976429	36.354650
1451.429654	79772.450089	36.359668
1453.346757	79887.489075	36.364685
1454.537244	80013.790286	36.369703
1456.029306	80125.577158	36.374720
1457.307336	80238.968752	36.379738
1458.226416	80362.197208	36.384756
1460.090076	80488.091739	36.389773
1461.444759	80624.606833	36.394791
1463.027747	80762.075263	36.399808
1464.660577	80883.547927	36.404826
1466.003818	81008.943021	36.409844
1467.585588	81137.278868	36.414861
1469.112967	81267.904279	36.419879
1470.668349	81391.278958	36.424896
1472.317157	81515.425153	36.429914
1474.329002	81648.396827	36.434932
1476.044705	81750.944553	36.439949
1477.799555	81870.540059	36.444967
1479.466036	81983.181428	36.449984
1481.116843	82103.909065	36.455002
1482.532750	82203.667053	36.460020
1484.162112	82324.639702	36.465037
1485.291753	82437.594505	36.470055
1486.880398	82559.398049	36.475072
1488.253577	82673.532217	36.480090
1489.635513	82788.717107	36.485108
1491.230865	82898.040945	36.490125
1492.987827	83026.624215	36.495143
1494.219793	83145.077489	36.500160
1495.910166	83253.779733	36.505178
1497.110582	83376.280735	36.510196
1498.734427	83489.124798	36.515213
1499.903291	83613.519636	36.520231
1501.628491	83740.653969	36.525248
1503.222003	83858.597800	36.530266
1504.513302	83996.976329	36.535284
1506.181186	84107.699979	36.540301
1507.653662	84229.693485	36.545319
1509.269653	84345.912600	36.550336
1510.828226	84470.453248	36.555354
1512.395162	84588.644977	36.560372
1514.139391	84709.863316	36.565389
1515.336002	84827.264708	36.570407
1516.608720	84952.067347	36.575424
1518.452087	85065.745105	36.580442
1520.136649	85189.939815	36.585460
1521.696068	85313.825085	36.590477
1523.181408	85429.308643	36.595495
1524.536260	85557.319643	36.600512
1526.394740	85665.510700	36.605530
1527.694045	85795.520820	36.610548
1529.020255	85908.838892	36.615565
1530.757985	86023.943413	36.620583
1531.782951	86159.142536	36.625600
1533.555678	86267.716671	36.630618
1534.803461	86395.608654	36.635636
1536.747320	86512.267001	36.640653
1538.544529	86628.479783	36.645671
1539.511078	86745.139115	36.650688
1541.281975	86852.334481	36.655706
1542.348418	86962.503760	36.660724
1544.314708	87056.452559	36.665741
1545.469171	87177.418215	36.670759
1547.094638	87291.708868	36.675776
1548.592092	87381.195052	36.680794
1549.911104	87509.625740	36.685812
1552.177309	87610.486709	36.690829
1553.330935	87729.769364	36.695847
1554.804358	87841.526015	36.700864
1556.323559	87961.411677	36.705882
1557.617422	88093.219705	36.710900
1559.041260	88208.863257	36.715917
1560.402264	88334.566419	36.720935
1562.098989	88473.993048	36.725952
1563.769218	88596.544395	36.730970
1565.307042	88725.060390	36.735988
1567.058204	88848.031058	36.741005
1568.606008	88984.682583	36.746023
1569.918452	89120.053385	36.751040
1571.882221	89240.736811	36.756058
1573.296498	89385.635741	36.761076
1574.829152	89520.758655	36.766093
1576.079328	89646.991565	36.771111
1577.438458	89793.510558	36.776128
1579.631357	89932.017715	36.781146
1581.482167	90068.246864	36.786164
1582.935232	90207.770260	36.791181
1584.463987	90340.920448	36.796199
1585.611819	90489.009230	36.801216
1587.517912	90620.505068	36.806234
1588.757868	90773.384203	36.811252
1590.791501	90914.379388	36.816269
1592.654748	91045.795044	36.821287
1594.333971	91191.016356	36.826304
1596.211293	91317.222068	36.831322
1597.705185	91465.071691	36.836340
1599.451776	91593.022561	36.841357
1601.381845	91723.442204	36.846375
1602.581556	91868.095032	36.851392
1604.820196	91991.636465	36.856410
1606.261390	92126.772678	36.861428
1607.721739	92248.218305	36.866445
1609.585694	92383.720789	36.871463
1611.024687	92515.994682	36.876480
1612.765553	92657.360431	36.881498
1614.286957	92787.125814	36.886516
1615.806799	92916.156869	36.891533
1617.610730	93052.318075	36.896551
1619.004017	93183.334520	36.901568
1620.865628	93318.562686	36.906586
1622.501624	93455.778479	36.911604
1624.208876	93575.669998	36.916621
1626.099281	93708.651965	36.921639
1627.654506	93846.946770	36.926656
1629.503611	93973.687577	36.931674
1630.874795	94102.036970	36.936692
1632.482676	94220.552220	36.941709
1634.027726	94350.814877	36.946727
1635.676111	94493.686487	36.951744
1637.193649	94616.007202	36.956762
1638.797240	94751.408586	36.961780
1640.614338	94881.948024	36.966797
1641.965583	95017.529277	36.971815
1642.882723	95162.406424	36.976832
1644.994985	95297.477516	36.981850
1646.439173	95428.089969	36.986868
1648.078095	95544.780180	36.991885
1649.577704	95674.231560	36.996903
1650.616010	95812.095904	37.001920
1652.604629	95924.841664	37.006938
1654.239834	96054.248167	37.011956
1656.441113	96181.602340	37.016973
1658.167958	96304.340780	37.021991
1659.214298	96437.022177	37.027008
1660.605676	96569.003954	37.032026
1662.617222	96704.299632	37.037044
1663.876744	96842.767889	37.042061
1665.381919	96978.599901	37.047079
1666.795989	97122.267929	37.052096
1668.642394	97260.329774	37.057114
1670.372559	97409.882430	37.062132
1672.021448	97557.546979	37.067149
1673.551720	97694.252841	37.072167
1675.405391	97853.308416	37.077184
1677.292998	97998.922299	37.082202
1679.266738	98148.009529	37.087220
1681.013582	98292.024053	37.092237
1682.888548	98443.168994	37.097255
1684.605900	98594.427923	37.102272
1686.383269	98740.518728	37.107290
1687.980993	98878.106568	37.112308
1689.535484	99030.952179	37.117325
1691.585855	99178.561771	37.122343
1693.064264	99332.954592	37.127360
1694.816332	99472.815530	37.132378
1696.686283	99621.735640	37.137396
1697.988091	99777.539906	37.142413
1700.159397	99925.235529	37.147431
1701.468698	100092.868143	37.152448
1703.248236	100236.658131	37.157466
1705.045191	100375.869454	37.162484
1706.833407	100539.068769	37.167501
1708.786106	100690.681268	37.172519
1709.920097	100851.549867	37.177536
1711.767586	101002.077235	37.182554
1713.786819	101160.616327	37.187572
1715.137991	101315.938556	37.192589
1717.475853	101475.469181	37.197607
1719.033248	101626.868656	37.202624
1720.342101	101777.090419	37.207642
1722.695977	101930.624038	37.212660
1724.089147	102091.458414	37.217677
1726.022669	102239.455135	37.222695
1727.585360	102407.605396	37.227712
1729.637656	102565.119209	37.232730
1731.556865	102711.193167	37.237748
1733.332398	102869.157220	37.242765
1735.352256	102997.099190	37.247783
1737.085494	103147.311878	37.252800
1738.702900	103291.280011	37.257818
1740.825483	103448.799783	37.262836
1742.430252	103595.649278	37.267853
1744.199805	103732.951964	37.272871
1745.778364	103878.729089	37.277888
1747.764072	104029.882757	37.282906
1749.524427	104176.178085	37.287924
1751.138590	104323.384344	37.292941
1753.091924	104463.818528	37.297959
1754.621321	104613.486328	37.302976
1755.964779	104750.694693	37.307994
1758.497915	104897.240601	37.313012
1760.267749	105032.545263	37.318029
1762.351330	105172.226745	37.323047
1763.565237	105305.628367	37.328064
1765.407547	105429.524533	37.333082
1766.976033	105545.260117	37.338100
1768.500174	105679.743413	37.343117
1769.817088	105805.016048	37.348135
1771.301078	105942.105961	37.353152
1773.058721	106083.883377	37.358170
1774.922570	106214.981161	37.363188
1776.246656	106364.003983	37.368205
1777.962779	106504.255358	37.373223
1779.591533	106655.577819	37.378240
1781.111966	106810.201932	37.383258
1783.123606	106966.791784	37.388276
1784.191794	107132.734958	37.393293
1786.322896	107288.889250	37.398311
1787.648863	107451.585765	37.403328
1789.609351	107618.609719	37.408346
1791.578134	107789.386583	37.413364
1793.081968	107975.237606	37.418381
1795.078394	108139.608288	37.423399
1796.940084	108322.958155	37.428416
1798.380485	108491.918652	37.433434
1800.396267	108659.585758	37.438452
1802.284603	108845.901528	37.443469
1804.032889	109027.256534	37.448487
1805.970795	109214.289372	37.453504
1807.689890	109396.639956	37.458522
1810.068512	109563.253156	37.463540
1811.821557	109746.462594	37.468557
1813.912809	109923.736302	37.473575
1815.721096	110092.000569	37.478592
1817.701831	110259.706191	37.483610
1820.000583	110427.325074	37.488628
1821.766203	110613.212841	37.493645
1823.456773	110775.563810	37.498663
1825.497660	110950.567877	37.503680
1827.263670	111115.470334	37.508698
1829.113137	111297.100324	37.513716
1830.748127	111469.215307	37.518733
1832.783292	111642.422882	37.523751
1834.752575	111823.009692	37.528768
1836.877864	111992.324307	37.533786
1838.849820	112148.639237	37.538804
1840.598277	112318.648146	37.543821
1842.916450	112486.413245	37.548839
1844.691502	112654.720216	37.553856
1846.857626	112816.029961	37.558874
1848.889627	112964.793217	37.563892
1850.419555	113129.602222	37.568909
1852.289070	113292.317272	37.573927
1853.908681	113456.695296	37.578944
1855.601128	113614.556633	37.583962
1857.584672	113786.095831	37.588980
1858.834044	113950.876150	37.593997
1861.011437	114125.823762	37.599015
1862.805151	114295.593979	37.604032
1864.512283	114470.908142	37.609050
1866.824181	114643.579779	37.614068
1868.452195	114818.185003	37.619085
1870.608238	114980.304974	37.624103
1872.184189	115154.526735	37.629120
1874.337762	115328.583325	37.634138
1876.129909	115489.633391	37.639156
1878.126906	115671.414618	37.644173
1879.847782	115833.339735	37.649191
1881.663017	116001.034451	37.654208
1883.351813	116172.732174	37.659226
1885.464098	116338.428954	37.664244
1887.553364	116514.340237	37.669261
1889.219796	116665.179442	37.674279
1891.069828	116810.562121	37.679296
1892.702434	116962.993242	37.684314
1894.767516	117109.206103	37.689332
1896.329780	117255.015811	37.694349
1898.033075	117412.663453	37.699367
1899.679117	117569.458170	37.704384
1901.668673	117735.053419	37.709402
1903.759973	117895.141424	37.714420
1905.259229	118063.820518	37.719437
1906.844311	118239.361758	37.724455
1908.547903	118411.727030	37.729472
1910.344281	118597.358957	37.734490
1911.952813	118770.603180	37.739508
1913.548769	118964.703103	37.744525
1915.666528	119159.864397	37.749543
1917.706361	119355.761831	37.754560
1919.275013	119551.403806	37.759578
1921.123435	119743.362776	37.764596
1922.995823	119954.853272	37.769613
1925.102287	120145.150464	37.774631
1927.558038	120343.182665	37.779648
1929.429046	120544.592255	37.784666
1932.032667	120723.195651	37.789684
1933.962390	120934.340111	37.794701
1935.983672	121127.090910	37.799719
1938.305491	121314.024193	37.804736
1940.295108	121506.654954	37.809754
1942.258537	121691.184914	37.814772
1944.019194	121894.419979	37.819789
1946.193639	122075.430471	37.824807
1948.277575	122270.650808	37.829824
1950.204779	122459.059064	37.834842
1952.081566	122652.372667	37.839860
1953.749962	122841.457308	37.844877
1955.918248	123036.731745	37.849895
1958.266621	123228.959930	37.854912
1959.913176	123438.487449	37.859930
1962.286332	123628.798169	37.864948
1964.267956	123827.962038	37.869965
1965.864774	124022.505685	37.874983
1967.903289	124216.905421	37.880000
1969.775611	124412.575200	37.885018
1972.481263	124615.588360	37.890036
1974.469887	124803.985491	37.895053
1976.285171	124992.372424	37.900071
1978.014126	125188.296644	37.905088
1980.101810	125378.431752	37.910106
1982.028423	125569.518929	37.915124
1983.743867	125771.816657	37.920141
1985.799703	125967.833324	37.925159
1987.906328	126163.056462	37.930176
1989.749625	126357.065538	37.935194
1991.769231	126561.679567	37.940212
1993.792508	126761.587250	37.945229
1995.965450	126965.304041	37.950247
1997.950446	127167.059247	37.955264
1999.687807	127373.801901	37.960282
2001.630582	127563.221195	37.965300
2003.501393	127766.456109	37.970317
2005.524104	127972.066251	37.975335
2007.505177	128169.323016	37.980352
2009.688111	128376.280440	37.985370
2011.847184	128574.361467	37.990388
2014.040910	128778.857864	37.995405
2016.272947	128974.671074	38.000423
2017.976935	129171.950319	38.005440
2019.927360	129365.461987	38.010458
2021.869082	129540.959462	38.015476
2024.118515	129724.212701	38.020493
2025.883887	129900.919071	38.025511
2027.780975	130076.717533	38.030528
2029.308589	130267.583945	38.035546
2031.384445	130441.389477	38.040564
2033.217018	130653.348199	38.045581
2035.159889	130841.082063	38.050599
2036.911530	131032.475301	38.055616
2038.736674	131238.639627	38.060634
2040.307485	131446.214848	38.065652
2042.423532	131650.153501	38.070669
2043.974834	131874.317370	38.075687
2046.355300	132091.400119	38.080704
2048.409642	132329.356457	38.085722
2050.522663	132542.118254	38.090740
2052.820194	132765.637665	38.095757
2054.618100	132996.303553	38.100775
2056.484867	133217.735244	38.105792
2058.505695	133449.409295	38.110810
2060.661859	133675.150500	38.115828
2062.917137	133908.592291	38.120845
2064.780638	134141.043101	38.125863
2067.172713	134372.182029	38.130880
2069.190411	134613.366752	38.135898
2071.417367	134850.015553	38.140916
2073.775521	135076.925229	38.145933
2075.974220	135318.288612	38.150951
2078.164762	135549.629953	38.155968
2080.093514	135788.994884	38.160986
2082.316951	136018.658504	38.166004
2084.390826	136250.326139	38.171021
2086.422139	136494.488181	38.176039
2088.343112	136721.892916	38.181056
2090.463165	136961.259630	38.186074
2093.137668	137198.752038	38.191092
2095.742059	137432.487688	38.196109
2097.487659	137672.969651	38.201127
2100.140836	137902.690065	38.206144
2102.008348	138136.493201	38.211162
2103.993782	138362.906184	38.216180
2106.131215	138604.194927	38.221197
2108.579874	138836.959373	38.226215
2111.011729	139060.565164	38.231232
2112.726180	139296.999458	38.236250
2115.071321	139523.679338	38.241268
2117.086605	139749.066449	38.246285
2119.115899	139988.006003	38.251303
2121.474772	140215.930744	38.256320
2123.720752	140445.155910	38.261338
2125.605474	140682.205156	38.266356
2127.616623	140910.022352	38.271373
2129.595728	141146.589648	38.276391
2131.818996	141372.535847	38.281408
2134.226066	141617.300667	38.286426
2135.930585	141841.997241	38.291444
2138.263176	142086.116087	38.296461
2140.069208	142324.632446	38.301479
2142.265537	142552.339726	38.306496
2144.568206	142802.368256	38.311514
2146.536591	143037.360018	38.316532
2148.905949	143267.911948	38.321549
2151.231990	143505.972382	38.326567
2154.018114	143733.479121	38.331584
2156.007163	143960.654055	38.336602
2158.179832	144200.556597	38.341620
2160.500229	144426.324077	38.346637
2162.464443	144637.958574	38.351655
2164.798167	144836.743070	38.356672
2166.367432	145046.016610	38.361690
2168.500718	145254.568642	38.366708
2171.007699	145466.160228	38.371725
2173.014713	145684.151155	38.376743
2175.070676	145901.221568	38.381760
2176.943841	146108.726073	38.386778
2178.885340	146322.414591	38.391796
2180.631613	146532.339393	38.396813
2182.808918	146763.089546	38.401831
2185.142848	146985.743999	38.406848
2186.887258	147228.938684	38.411866
2188.990205	147454.905756	38.416884
2191.266981	147695.938209	38.421901
2193.093407	147929.718225	38.426919
2195.124028	148173.228173	38.431936
2197.226166	148426.526913	38.436954
2199.643206	148675.475007	38.441972
2201.718475	148921.583495	38.446989
2203.980972	149183.682447	38.452007
2206.179629	149436.742534	38.457024
2208.332035	149700.549332	38.462042
2210.440743	149958.741186	38.467060
2213.104114	150203.164734	38.472077
2215.295040	150476.654232	38.477095
2217.828216	150738.337867	38.482112
2219.658765	150997.707685	38.487130
2221.765342	151260.843803	38.492148
2224.579272	151515.252240	38.497165
2226.513353	151778.925433	38.502183
2229.435568	152041.125975	38.507200
2232.082176	152303.142171	38.512218
2234.275217	152560.711234	38.517236
2237.339280	152807.838600	38.522253
2239.491810	153072.956433	38.527271
2242.010600	153318.152599	38.532288
2243.842997	153556.106872	38.537306
2246.057200	153810.581075	38.542324
2248.470802	154055.060567	38.547341
2250.496183	154301.988021	38.552359
2252.831634	154550.493141	38.557376
2254.912024	154804.383299	38.562394
2257.265646	155068.603274	38.567412
2259.931804	155315.651179	38.572429
2262.273646	155569.783300	38.577447
2264.298351	155815.752591	38.582464
2266.778884	156067.097917	38.587482
2268.639213	156324.126445	38.592500
2271.175412	156577.686847	38.597517
2273.349677	156840.787574	38.602535
2275.580516	157086.907845	38.607552
2278.223920	157335.795863	38.612570
2279.679490	157608.482137	38.617588
2282.417464	157863.184562	38.622605
2284.599871	158126.708639	38.627623
2286.915485	158387.991518	38.632640
2289.125997	158637.840963	38.637658
2291.360545	158894.225665	38.642676
2294.122483	159140.297090	38.647693
2296.227290	159410.326039	38.652711
2298.641087	159662.585522	38.657728
2301.066423	159920.404785	38.662746
2303.366984	160170.614635	38.667764
2305.487443	160421.666028	38.672781
2307.695804	160678.836657	38.677799
2310.029180	160938.058256	38.682816
2312.140242	161194.192415	38.687834
2314.234806	161446.991237	38.692852
2316.133078	161681.019349	38.697869
2318.535231	161932.807369	38.702887
2320.986586	162164.199346	38.707904
2322.836269	162409.790829	38.712922
2324.728388	162651.961462	38.717940
2327.187854	162900.202220	38.722957
2329.197121	163157.616986	38.727975
2331.361016	163420.239458	38.732992
2333.878936	163677.335894	38.738010
2336.292272	163945.304778	38.743028
2338.634679	164213.133437	38.748045
2340.835325	164481.289952	38.753063
2343.300472	164735.897573	38.758080
2345.819829	165004.285912	38.763098
2348.306165	165266.014881	38.768116
2350.859077	165518.529617	38.773133
2353.094343	165800.017241	38.778151
2355.845271	166064.641006	38.783168
2358.335272	166328.823936	38.788186
2360.578565	166605.692093	38.793204
2363.190659	166864.043040	38.798221
2365.621690	167138.928836	38.803239
2368.361802	167392.614840	38.808256
2370.801808	167663.539928	38.813274
2372.907801	167933.730841	38.818292
2375.378580	168195.206741	38.823309
2377.731567	168467.938728	38.828327
2380.066352	168728.612459	38.833344
2382.631270	169005.592408	38.838362
2384.525246	169291.134099	38.843380
2387.080027	169564.245167	38.848397
2389.385186	169841.941702	38.853415
2391.568982	170120.686659	38.858432
2394.132170	170405.760365	38.863450
2396.324448	170688.442315	38.868468
2399.216603	170978.545971	38.873485
2401.410846	171252.214628	38.878503
2403.913206	171538.762362	38.883520
2406.840613	171819.239115	38.888538
2409.697444	172088.452457	38.893556
2412.378257	172364.042951	38.898573
2414.736037	172641.944897	38.903591
2417.451817	172913.595659	38.908608
2420.130053	173179.818586	38.913626
2422.432727	173442.469309	38.918644
2425.244867	173704.457532	38.923661
2427.834692	173972.665095	38.928679
2429.577850	174241.830700	38.933696
2432.118056	174501.933818	38.938714
2434.436454	174781.081215	38.943732
2436.653044	175042.912598	38.948749
2439.099265	175323.908606	38.953767
2441.316295	175602.300049	38.958784
2443.668499	175880.785693	38.963802
2445.832394	176174.552155	38.968820
2448.068253	176451.838818	38.973837
2450.904917	176729.642431	38.978855
2452.978895	177016.200543	38.983872
2455.523013	177296.819815	38.988890
2457.715356	177591.158286	38.993908
2460.397843	177875.110338	38.998925
2462.417499	178172.576129	39.003943
2464.799437	178470.977063	39.008960
2467.076827	178763.579336	39.013978
2469.290600	179064.725993	39.018996
2471.998073	179360.564995	39.024013
2474.391058	179656.174563	39.029031
2476.706592	179958.527529	39.034048
2479.071594	180236.542877	39.039066
2481.156375	180523.771276	39.044084
2483.583062	180792.076815	39.049101
2486.556729	181082.952934	39.054119
2488.450636	181361.146649	39.059136
2490.901829	181643.902322	39.064154
2493.338233	181938.090314	39.069172
2495.419485	182227.483452	39.074189
2498.043005	182530.711351	39.079207
2500.405977	182827.174013	39.084224
2503.122174	183122.896874	39.089242
2505.558266	183441.421313	39.094260
2508.115106	183735.240574	39.099277
2511.197673	184030.121852	39.104295
2513.220156	184344.675237	39.109312
2516.121659	184639.459533	39.114330
2518.514729	184953.322215	39.119348
2521.237475	185315.341877	39.124365
2523.537267	185645.959188	39.129383
2526.211629	185962.702136	39.134400
2528.556738	186282.570612	39.139418
2531.309931	186605.653085	39.144436
2533.901113	186919.897383	39.149453
2536.476693	187251.543693	39.154471
2538.876061	187568.054929	39.159488
2541.729800	187894.961043	39.164506
2543.676638	188223.584066	39.169524
2545.755274	188557.445329	39.174541
2548.985711	188895.928938	39.179559
2551.328472	189238.387118	39.184576
2554.395862	189567.576370	39.189594
2556.796583	189902.636154	39.194612
2559.147873	190235.164603	39.199629
2561.945735	190584.236278	39.204647
2564.489203	190917.549596	39.209664
2567.503900	191249.342708	39.214682
2570.283930	191589.225219	39.219700
2572.791792	191921.124485	39.224717
2575.136222	192254.751941	39.229735
2577.945753	192598.290396	39.234752
2580.491152	192933.361667	39.239770
2583.046711	193280.269040	39.244788
2585.578631	193620.754628	39.249805
2588.858604	193959.473656	39.254823
2591.332890	194303.500769	39.259840
2593.932601	194641.311413	39.264858
2596.432987	194980.967268	39.269876
2599.438573	195310.283286	39.274893
2602.317187	195635.174652	39.279911
2604.838434	195968.885872	39.284928
2607.860797	196300.462409	39.289946
2610.012833	196631.159124	39.294964
2612.654832	196961.221540	39.299981
2615.270468	197289.434513	39.304999
2618.164884	197636.097244	39.310016
2620.976882	197964.662223	39.315034
2623.421254	198305.147767	39.320052
2625.904554	198628.558019	39.325069
2628.447439	198959.504048	39.330087
2631.166019	199293.039852	39.335104
2633.567131	199622.282048	39.340122
2635.747902	199965.479538	39.345140
2638.326805	200303.586203	39.350157
2641.686583	200631.055580	39.355175
2643.868307	200977.735185	39.360192
2646.974029	201303.416490	39.365210
2649.381735	201642.416247	39.370228
2651.998370	201965.279090	39.375245
2654.832131	202277.312741	39.380263
2657.236278	202584.587349	39.385280
2659.770929	202875.559204	39.390298
2662.361807	203184.279138	39.395316
2664.678148	203486.894906	39.400333
2667.421507	203797.903786	39.405351
2670.050119	204120.717869	39.410368
2672.713996	204432.070409	39.415386
2674.761578	204751.013167	39.420404
2677.327428	205078.080890	39.425421
2680.388120	205416.782842	39.430439
2682.566888	205748.560621	39.435456
2685.230788	206080.161833	39.440474
2687.893826	206415.294717	39.445492
2690.467343	206766.420537	39.450509
2693.288737	207105.162491	39.455527
2695.722159	207464.160775	39.460544
2698.826762	207811.928633	39.465562
2701.389687	208161.965990	39.470580
2703.755414	208518.588583	39.475597
2706.644028	208886.409367	39.480615
2709.489348	209245.447925	39.485632
2712.468353	209607.946452	39.490650
2715.086585	209961.407255	39.495668
2717.364997	210331.586026	39.500685
2720.132830	210698.386712	39.505703
2722.666154	211085.623341	39.510720
2725.562341	211451.007872	39.515738
2728.379558	211829.487960	39.520756
2730.879988	212218.509493	39.525773
2734.060417	212595.384421	39.530791
2737.053953	212970.358220	39.535808
2739.998647	213345.035219	39.540826
2743.293242	213709.979405	39.545844
2745.707382	214081.894589	39.550861
2748.879701	214453.768394	39.555879
2751.792134	214827.359672	39.560896
2754.635070	215202.029098	39.565914
2757.603955	215568.778715	39.570932
2760.344817	215939.450933	39.575949
2763.257451	216299.960629	39.580967
2765.620098	216676.408212	39.585984
2768.818911	217049.753735	39.591002
2771.536182	217419.313105	39.596020
2774.117855	217795.397255	39.601037
2777.055412	218167.234652	39.606055
2780.099744	218535.676969	39.611072
2782.618641	218916.877866	39.616090
2785.652458	219283.086748	39.621108
2788.035122	219657.374025	39.626125
2791.030612	220030.956449	39.631143
2793.672547	220411.173729	39.636160
2796.070331	220797.958026	39.641178
2798.917485	221168.083743	39.646196
2801.177047	221564.924492	39.651213
2804.519549	221951.562278	39.656231
2807.675571	222331.014470	39.661248
2810.282807	222715.099513	39.666266
2813.539211	223091.919696	39.671284
2816.281927	223466.533544	39.676301
2819.138638	223844.178223	39.681319
2822.561094	224210.430108	39.686336
2825.391976	224583.480787	39.691354
2828.362446	224963.089444	39.696372
2830.940995	225336.509713	39.701389
2833.885542	225703.013934	39.706407
2836.214375	226077.616266	39.711424
2839.130070	226436.859398	39.716442
2841.773371	226787.863164	39.721460
2844.846189	227114.361322	39.726477
2847.865995	227456.669038	39.731495
2850.221803	227802.839841	39.736512
2853.082058	228146.594908	39.741530
2855.547034	228483.831764	39.746548
2857.777118	228841.961839	39.751565
2860.676019	229192.010863	39.756583
2863.271425	229567.307835	39.761600
2865.656067	229937.810706	39.766618
2868.965223	230304.740022	39.771636
2871.559238	230682.170724	39.776653
2874.488003	231052.791693	39.781671
2877.573414	231432.406529	39.786688
2880.382264	231814.630005	39.791706
2883.434682	232192.674514	39.796724
2886.016391	232586.415482	39.801741
2888.691809	232988.220060	39.806759
2891.905524	233382.649660	39.811776
2894.603191	233781.808189	39.816794
2897.107705	234175.636246	39.821812
2900.219197	234587.177632	39.826829
2903.068680	234993.881889	39.831847
2906.059301	235411.970119	39.836864
2908.814314	235827.986088	39.841882
2911.923880	236242.015771	39.846900
2914.613581	236662.004017	39.851917
2917.770550	237077.829083	39.856935
2920.256890	237506.866325	39.861952
2923.447588	237936.199886	39.866970
2925.757430	238368.311950	39.871988
2929.440453	238807.805415	39.877005
2932.434130	239236.227982	39.882023
2935.569334	239677.913949	39.887040
2938.366926	240110.379527	39.892058
2941.705983	240543.293658	39.897076
2944.662353	240977.206589	39.902093
2948.064363	241404.317585	39.907111
2951.024262	241840.921306	39.912128
2953.657577	242270.512993	39.917146
2957.100153	242691.518732	39.922164
2960.204651	243131.984363	39.927181
2963.558837	243551.020891	39.932199
2966.648481	243976.219960	39.937216
2969.777257	244408.397964	39.942234
2972.884420	244822.212130	39.947252
2975.726530	245248.387161	39.952269
2978.717369	245672.607562	39.957287
2981.907377	246102.613337	39.962304
2984.949149	246519.863669	39.967322
2988.625668	246922.433186	39.972340
2991.542190	247339.269409	39.977357
2994.609805	247741.627122	39.982375
2997.856351	248158.130738	39.987392
3000.627476	248567.112043	39.992410
3004.341117	248969.874563	39.997428
3006.798539	249379.029826	40.002445
3009.608752	249790.034394	40.007463
3012.710656	250191.288918	40.012480
3015.432234	250603.321384	40.017498
3018.945328	251007.100967	40.022516
3021.885077	251422.704512	40.027533
3024.714921	251824.429187	40.032551
3027.707295	252237.507601	40.037568
3030.233012	252654.061375	40.042586
3033.246103	253067.591556	40.047604
3035.969186	253484.137724	40.052621
3038.932167	253888.554200	40.057639
3041.932144	254292.074737	40.062656
3044.541079	254682.497012	40.067674
3048.081646	255064.517765	40.072692
3050.242801	255455.413992	40.077709
3052.862245	255858.938434	40.082727
3056.237527	256251.091318	40.087744
3058.584885	256664.384351	40.092762
3061.869593	257077.073006	40.097780
3064.636559	257497.918431	40.102797
3067.449220	257911.770124	40.107815
3070.329616	258330.182071	40.112832
3072.994346	258772.325050	40.117850
3076.375176	259207.090434	40.122868
3079.144965	259653.125589	40.127885
3082.519438	260097.337764	40.132903
3084.985892	260552.129120	40.137920
3088.090660	261000.443922	40.142938
3091.710567	261464.399510	40.147956
3094.744036	261912.950452	40.152973
3097.967615	262369.115408	40.157991
3101.617263	262832.197147	40.163008
3104.633642	263296.975666	40.168026
3108.038577	263751.557287	40.173044
3111.399178	264210.588797	40.178061
3114.247971	264678.714750	40.183079
3117.878789	265136.582606	40.188096
3120.539807	265603.971646	40.193114
3124.409629	266055.321438	40.198132
3127.699372	266520.982891	40.203149
3131.100497	266970.064815	40.208167
3135.025923	267428.867012	40.213184
3137.865313	267879.098949	40.218202
3141.626637	268321.159410	40.223220
3144.618837	268765.090006	40.228237
3147.924234	269224.462706	40.233255
3151.212176	269675.378305	40.238272
3154.315506	270118.218487	40.243290
3157.356767	270564.418713	40.248308
3160.720418	271012.065050	40.253325
3163.761001	271462.426187	40.258343
3167.169890	271914.607151	40.263360
3170.041665	272371.440907	40.268378
3173.270247	272832.229513	40.273396
3176.016835	273279.579428	40.278413
3179.238944	273740.465778	40.283431
3182.433182	274200.668252	40.288448
3184.890992	274673.554158	40.293466
3188.513010	275135.945230	40.298484
3191.405617	275618.713526	40.303501
3194.429306	276087.287484	40.308519
3198.212336	276553.302544	40.313536
3201.143758	277035.269085	40.318554
3204.250957	277497.168086	40.323572
3207.615277	277978.121880	40.328589
3210.843129	278465.087278	40.333607
3214.126952	278941.120920	40.338624
3217.239642	279419.413012	40.343642
3220.292312	279892.581645	40.348660
3223.491733	280372.454101	40.353677
3226.702838	280859.508343	40.358695
3230.372116	281345.472303	40.363712
3233.274466	281830.003333	40.368730
3236.363559	282298.681517	40.373748
3239.350892	282786.544954	40.378765
3242.581695	283275.611472	40.383783
3246.275877	283761.072793	40.388800
3249.366665	284243.298114	40.393818
3252.780349	284714.931636	40.398836
3256.439973	285163.746039	40.403853
3259.082517	285610.100303	40.408871
3262.354715	286043.124012	40.413888
3265.414846	286501.900685	40.418906
3268.921520	286936.888178	40.423924
3271.920479	287380.737573	40.428941
3275.060823	287847.313326	40.433959
3278.263523	288293.689471	40.438976
3281.446990	288759.490250	40.443994
3284.786437	289213.634062	40.449012
3288.338573	289681.935356	40.454029
3291.292429	290151.316568	40.459047
3294.918239	290608.249699	40.464064
3297.733086	291087.827374	40.469082
3300.938868	291551.395209	40.474100
3304.651762	292034.659819	40.479117
3307.678793	292515.691458	40.484135
3311.107095	293001.861823	40.489152
3314.217635	293484.904007	40.494170
3317.276186	293974.551709	40.499188
3320.939007	294461.968655	40.504205
3324.000395	294967.907752	40.509223
3327.880234	295461.046036	40.514240
3330.928379	295965.836085	40.519258
3334.175747	296480.466890	40.524276
3337.599397	296983.818641	40.529293
3340.957290	297503.043757	40.534311
3344.110832	298008.078724	40.539328
3347.516365	298522.768033	40.544346
3351.065418	299042.990120	40.549364
3354.235546	299561.311493	40.554381
3357.672745	300089.614276	40.559399
3361.325614	300614.958939	40.564416
3364.516913	301133.922205	40.569434
3368.276404	301656.930019	40.574452
3371.479398	302185.807330	40.579469
3375.212862	302715.866130	40.584487
3378.682795	303226.439237	40.589504
3382.241697	303761.160235	40.594522
3385.963531	304286.153366	40.599540
3389.362584	304804.794477	40.604557
3392.528819	305319.075096	40.609575
3396.334356	305837.236379	40.614592
3399.895725	306374.620601	40.619610
3403.589767	306889.691643	40.624628
3407.233021	307399.384029	40.629645
3410.660903	307920.298673	40.634663
3414.070196	308436.717974	40.639680
3417.407240	308955.833658	40.644698
3421.247429	309461.362156	40.649716
3424.421413	309976.837303	40.654733
3428.098558	310490.908806	40.659751
3431.536450	311001.230199	40.664768
3435.183456	311512.275036	40.669786
3438.815697	312022.504481	40.674804
3442.180705	312529.191320	40.679821
3445.417677	313041.273258	40.684839
3448.964780	313537.540258	40.689856
3452.336356	314041.011761	40.694874
3455.942082	314560.481223	40.699892
3459.633328	315065.795230	40.704909
3462.454220	315581.542950	40.709927
3466.162282	316092.654717	40.714944
3469.863322	316598.787607	40.719962
3472.918916	317111.359756	40.724980
3476.565072	317611.678122	40.729997
3480.095302	318126.245692	40.735015
3483.689083	318606.709199	40.740020
3486.689555	319074.859626	40.745024
3489.579983	319492.495030	40.750029
3493.259738	319850.954004	40.755034
3495.648047	320185.848838	40.760039
3498.567087	320464.433696	40.765044
3500.557780	320707.467567	40.770048
3502.744012	320912.257520	40.775053
3505.033080	321064.240984	40.780058
3506.522172	321198.056562	40.785063
3508.456215	321272.475003	40.790068
3509.989260	321327.162944	40.795072
3510.961995	321349.755697	40.800077
3512.227850	321343.275140	40.805082
3513.200713	321326.333216	40.810087
3514.182139	321265.199618	40.815092
3514.926727	321192.196559	40.820096
3515.613264	321100.808774	40.825101
3516.249091	320992.078076	40.830106
3516.365661	320873.022597	40.835111
3517.158709	320721.449771	40.840116
3517.835633	320582.055293	40.845120
3517.760319	320417.972334	40.850125
3518.111834	320251.710709	40.855130
3517.800574	320078.326245	40.860135
3518.108205	319894.159379	40.865140
3518.168463	319720.054191	40.870144
3518.116872	319520.753042	40.875149
3518.221222	319316.974404	40.880154
3517.812250	319125.054285	40.885159
3518.036705	318905.506509	40.890164
3517.767653	318715.827160	40.895168
3518.322638	318503.298844	40.900173
3518.030902	318296.981987	40.905178
3518.124805	318083.531144	40.910183
3517.849968	317862.631081	40.915188
3517.643618	317655.839976	40.920192
3517.341658	317435.043773	40.925197
3517.521250	317228.368721	40.930202
3516.724248	317016.069099	40.935207
3516.620261	316797.554254	40.940212
3516.241704	316605.949232	40.945216
3516.355792	316395.794791	40.950221
3516.302020	316189.507469	40.955226
3516.231188	315982.407661	40.960231
3515.916954	315785.293303	40.965236
3515.628491	315581.177004	40.970240
3515.116648	315383.684548	40.975245
3514.728154	315180.523444	40.980250
3514.169126	314998.812019	40.985255
3514.399504	314813.694711	40.990260
3514.252174	314632.095874	40.995264
3513.837774	314446.695754	41.000269
3514.062192	314263.892609	41.005274
3513.659589	314093.323450	41.010279
3513.792010	313905.011693	41.015284
3513.351465	313730.859379	41.020288
3513.281364	313559.854838	41.025293
3513.219549	313383.632129	41.030298
3512.671434	313226.390219	41.035303
3512.731209	313036.661316	41.040308
3512.520188	312883.767834	41.045312
3512.085792	312715.666771	41.050317
3512.125420	312551.384514	41.055322
3511.578108	312394.292357	41.060327
3511.872848	312234.142381	41.065332
3511.462306	312085.577681	41.070336
3511.171536	311933.253328	41.075341
3511.339965	311792.562181	41.080346
3510.929976	311649.008883	41.085351
3511.079084	311496.309322	41.090356
3511.003223	311349.929497	41.095360
3510.760965	311208.867945	41.100365
3510.401994	311057.594696	41.105370
3510.307002	310925.899104	41.110375
3510.307925	310789.251600	41.115380
3510.395535	310646.024996	41.120384
3510.015004	310511.675362	41.125389
3510.271479	310369.541311	41.130394
3509.579992	310243.204144	41.135399
3509.865717	310113.304700	41.140404
3509.269406	309991.354373	41.145408
3509.377032	309860.489534	41.150413
3509.248319	309728.999495	41.155418
3508.961010	309606.440280	41.160423
3509.244350	309488.296111	41.165428
3509.060604	309359.460146	41.170432
3509.007845	309228.007830	41.175437
3508.670140	309118.916871	41.180442
3508.843723	309008.957236	41.185447
3508.596370	308883.336294	41.190452
3508.594575	308763.478866	41.195456
3508.230891	308660.065739	41.200461
3508.483227	308544.545225	41.205466
3508.297258	308431.510183	41.210471
3508.116444	308322.138564	41.215476
3508.235605	308216.231827	41.220480
3508.258327	308098.862860	41.225485
3508.258211	307983.507560	41.230490
3508.018515	307882.745550	41.235495
3507.721458	307772.703709	41.240500
3507.693935	307671.119363	41.245504
3507.448962	307567.812721	41.250509
3507.723240	307459.055484	41.255514
3507.385454	307356.246364	41.260519
3507.406964	307259.641417	41.265524
3507.283148	307158.529082	41.270528
3506.700304	307068.176323	41.275533
3507.158273	306959.669349	41.280538
3507.119008	306873.710589	41.285543
3506.878174	306773.480939	41.290548
3506.956213	306686.943737	41.295552
3506.700284	306599.440408	41.300557
3506.526122	306502.966250	41.305562
3506.614279	306424.137989	41.310567
3506.876711	306331.209290	41.315572
3506.553553	306233.205425	41.320576
3506.471059	306155.115869	41.325581
3506.233119	306066.565414	41.330586
3506.251553	305982.224892	41.335591
3506.109174	305887.678741	41.340596
3506.491525	305807.276799	41.345600
3506.216503	305720.411152	41.350605
3506.434231	305627.818963	41.355610
3506.144146	305546.630529	41.360615
3506.390160	305466.452860	41.365620
3506.183697	305383.062518	41.370624
3506.445814	305308.226447	41.375629
3506.782659	305218.414408	41.380634
3506.267458	305129.880025	41.385639
3506.385302	305044.071870	41.390644
3506.039600	304955.358114	41.395648
3505.972786	304882.583120	41.400653
3506.108471	304789.035103	41.405658
3506.091737	304717.397315	41.410663
3505.739265	304630.872722	41.415668
3505.896056	304541.392918	41.420672
3505.828795	304466.021538	41.425677
3506.004440	304385.115094	41.430682
3505.722997	304303.236211	41.435687
3505.907949	304232.533461	41.440692
3505.677414	304158.866733	41.445696
3505.613954	304088.991391	41.450701
3505.550986	304003.285998	41.455706
3505.095236	303925.098440	41.460711
3505.516206	303856.521704	41.465716
3505.791596	303783.081117	41.470720
3505.696681	303712.370313	41.475725
3505.845295	303623.526459	41.480730
3505.430881	303561.340071	41.485735
3505.426937	303480.714674	41.490740
3505.681664	303407.556729	41.495744
3505.724847	303328.730734	41.500749
3505.745053	303252.198727	41.505754
3505.274527	303180.858498	41.510759
3505.658535	303100.630255	41.515764
3505.735945	303024.954331	41.520768
3505.349348	302959.530696	41.525773
3505.584970	302884.415311	41.530778
3505.421452	302808.572964	41.535783
3505.691780	302737.396806	41.540788
3505.420907	302660.578380	41.545792
3505.281577	302580.023577	41.550797
3505.447119	302502.729800	41.555802
3504.987506	302435.764388	41.560807
3505.063928	302365.559583	41.565812
3505.370332	302292.086646	41.570816
3505.059235	302237.212451	41.575821
3505.322846	302157.637790	41.580826
3505.277224	302095.748602	41.585831
3505.596768	302016.954005	41.590836
3505.445173	301953.070520	41.595840
3505.222781	301878.839420	41.600845
3505.632436	301810.185444	41.605850
3504.858276	301735.734596	41.610855
3505.002674	301668.419719	41.615860
3505.152256	301600.340418	41.620864
3504.771549	301538.859047	41.625869
3505.360370	301467.275320	41.630874
3505.212398	301397.893153	41.635879
3504.805678	301326.438707	41.640884
3504.584184	301260.020149	41.645888
3504.691514	301203.094584	41.650893
3504.893034	301129.814539	41.655898
3504.797958	301079.512240	41.660903
3505.121984	301006.594735	41.665908
3504.869093	300932.239822	41.670912
3504.831214	300878.441588	41.675917
3504.702157	300802.667396	41.680922
3504.890866	300741.910959	41.685927
3504.507076	300674.371620	41.690932
3504.887457	300618.853692	41.695936
3504.211091	300551.410632	41.700941
3504.730597	300482.228845	41.705946
3504.237941	300436.823634	41.710951
3504.767216	300372.552361	41.715956
3504.695214	300312.777729	41.720960
3504.350902	300244.875391	41.725965
3504.984018	300179.875084	41.730970
3504.920281	300124.527572	41.735975
3504.474930	300057.862413	41.740980
3504.402162	299996.127762	41.745984
3504.754305	299929.847385	41.750989
3504.994484	299865.696862	41.755994
3504.590126	299801.748370	41.760999
3504.526839	299732.401810	41.766004
3504.624184	299682.348254	41.771008
3504.265766	299621.701167	41.776013
3504.301034	299563.945193	41.781018
3504.571217	299503.531035	41.786023
3504.432056	299436.613860	41.791028
3504.148705	299370.788033	41.796032
3504.263393	299319.229773	41.801037
3504.329803	299261.188662	41.806042
3504.261083	299202.710379	41.811047
3504.447686	299150.529917	41.816052
3504.588381	299090.619053	41.821056
3504.139278	299028.840076	41.826061
3504.520599	298965.328308	41.831066
3504.513926	298913.737652	41.836071
3504.473244	298855.941856	41.841076
3504.601697	298792.571050	41.846080
3504.137451	298735.757328	41.851085
3504.571624	298676.563925	41.856090
3504.229972	298611.204417	41.861095
3504.415775	298555.383814	41.866100
3504.347236	298500.035428	41.871104
3504.335303	298446.739839	41.876109
3504.249390	298374.620775	41.881114
3504.053655	298326.546008	41.886119
3504.133121	298270.334427	41.891124
3504.564359	298215.264327	41.896128
3504.036525	298148.533354	41.901133
3504.620686	298089.748690	41.906138
3504.409276	298048.573819	41.911143
3504.269459	297972.491997	41.916148
3504.198965	297919.306833	41.921152
3504.126879	297863.194788	41.926157
3504.389491	297812.681143	41.931162
3503.838899	297753.919995	41.936167
3504.100627	297695.566889	41.941172
3504.292210	297648.271220	41.946176
3503.987199	297594.333203	41.951181
3503.894306	297540.540297	41.956186
3504.189889	297482.588953	41.961191
3504.001298	297432.450619	41.966196
3503.965033	297368.442067	41.971200
3504.176275	297315.008871	41.976205
3504.115902	297259.047125	41.981210
3504.025172	297203.548206	41.986215
3504.108999	297142.982341	41.991220
3503.897352	297103.155840	41.996224
3503.737775	297053.496269	42.001229
3503.856994	296995.495515	42.006234
3503.937257	296939.435213	42.011239
3503.774249	296894.892144	42.016244
3503.757168	296838.795985	42.021248
3503.746172	296787.993117	42.026253
3504.073694	296727.287078	42.031258
3503.629573	296678.256887	42.036263
3504.016449	296636.809722	42.041268
3503.883691	296582.411237	42.046272
3504.188717	296530.897177	42.051277
3503.837011	296468.183925	42.056282
3503.966793	296423.111313	42.061287
3503.725722	296374.023813	42.066292
3503.982734	296323.357005	42.071296
3503.663161	296274.968882	42.076301
3504.146505	296221.339606	42.081306
3504.025257	296167.498918	42.086311
3503.969631	296116.015157	42.091316
3503.871701	296058.327242	42.096320
3503.785304	296015.120615	42.101325
3503.755216	295950.982257	42.106330
3503.531615	295902.757065	42.111335
3503.670142	295857.657199	42.116340
3503.796710	295805.915728	42.121344
3503.598682	295761.555411	42.126349
3503.855707	295708.240871	42.131354
3503.775975	295653.451457	42.136359
3503.297521	295608.472862	42.141364
3503.905199	295556.783572	42.146368
3503.869806	295509.368745	42.151373
3503.944517	295452.187897	42.156378
3503.782964	295396.876442	42.161383
3504.114796	295340.648177	42.166388
3504.066519	295304.154939	42.171392
3503.643867	295256.723808	42.176397
3504.167323	295198.836532	42.181402
3503.833915	295140.573458	42.186407
3503.792221	295085.675777	42.191412
3503.966712	295035.886132	42.196416
3503.707139	295004.592769	42.201421
3503.997523	294938.698008	42.206426
3503.546284	294888.191077	42.211431
3503.711787	294838.911748	42.216436
3503.731033	294781.764333	42.221440
3503.757745	294742.866382	42.226445
3503.685257	294691.053088	42.231450
3503.660527	294641.523200	42.236455
3503.530524	294593.842361	42.241460
3503.925435	294545.927075	42.246464
3503.508163	294489.483664	42.251469
3503.588131	294441.871846	42.256474
3503.970691	294388.969302	42.261479
3504.139645	294341.521738	42.266484
3503.859188	294286.507744	42.271488
3503.652030	294233.340468	42.276493
3503.741379	294187.050617	42.281498
3503.967439	294138.906735	42.286503
3503.648480	294077.942191	42.291508
3503.875708	294023.968951	42.296512
3503.836351	293988.848059	42.301517
3503.785438	293934.052566	42.306522
3503.693094	293893.136222	42.311527
3503.992562	293839.635211	42.316532
3503.853157	293780.195154	42.321536
3503.844969	293730.763755	42.326541
3504.191228	293678.858963	42.331546
3503.799128	293625.338106	42.336551
3503.723880	293576.426108	42.341556
3503.439584	293518.611987	42.346560
3503.544434	293477.995585	42.351565
3503.679000	293419.861641	42.356570
3503.650728	293385.273222	42.361575
3503.733801	293325.339908	42.366580
3503.714289	293288.077314	42.371584
3503.790164	293226.821371	42.376589
3503.621572	293173.367151	42.381594
3503.550019	293126.668789	42.386599
3503.454393	293078.345023	42.391604
3503.512459	293029.131833	42.396608
3503.440118	292984.011691	42.401613
3503.693661	292933.291616	42.406618
3503.524622	292892.081067	42.411623
3503.569173	292844.575316	42.416628
3503.793607	292791.823251	42.421632
3503.596958	292750.820543	42.426637
3503.906458	292700.829764	42.431642
3503.812591	292655.101807	42.436647
3503.357117	292601.717181	42.441652
3503.686010	292554.854246	42.446656
3503.404270	292511.140917	42.451661
3503.291989	292454.215399	42.456666
3503.416579	292416.904391	42.461671
3503.279524	292368.484688	42.466676
3503.202334	292321.710221	42.471680
3503.064433	292290.701973	42.476685
3503.344984	292248.835557	42.481690
3503.286297	292204.349097	42.486695
3503.329023	292162.239622	42.491700
3503.312143	292107.488094	42.496704
3503.240672	292070.232840	42.501709
3503.466479	292026.083810	42.506714
3503.308911	291988.129154	42.511719
3503.061464	291942.195465	42.516724
3503.101706	291898.940704	42.521728
3503.222554	291860.382625	42.526733
3503.284518	291815.597099	42.531738
3503.182965	291771.269729	42.536743
3503.446431	291731.263870	42.541748
3503.432757	291684.071747	42.546752
3503.048115	291637.471882	42.551757
3503.281716	291587.339276	42.556762
3502.897184	291550.997914	42.561767
3502.861893	291517.351387	42.566772
3503.062760	291475.929592	42.571776
3502.884965	291426.039064	42.576781
3503.394299	291381.539986	42.581786
3503.147050	291348.308186	42.586791
3503.423966	291309.343644	42.591796
3503.331625	291265.803604	42.596800
3503.298861	291231.469226	42.601805
3503.307933	291178.952940	42.606810
3503.057454	291135.590152	42.611815
3503.149576	291091.613995	42.616820
3503.258381	291059.675789	42.621824
3503.128809	291012.883029	42.626829
3503.357697	290971.303804	42.631834
3503.397122	290917.458873	42.636839
3503.257706	290880.748051	42.641844
3503.377294	290833.356355	42.646848
3502.816788	290797.067393	42.651853
3502.950292	290751.531750	42.656858
3503.592966	290712.789935	42.661863
3503.005877	290673.781256	42.666868
3503.051663	290632.535771	42.671872
3502.624964	290591.465607	42.676877
3502.685429	290541.817312	42.681882
3502.870167	290517.809278	42.686887
3502.984408	290483.731630	42.691892
3503.118693	290446.239739	42.696896
3502.699924	290406.771950	42.701901
3503.201762	290363.291558	42.706906
3503.322280	290314.041036	42.711911
3502.781848	290275.152130	42.716916
3502.956402	290233.962715	42.721920
3502.567078	290196.730349	42.726925
3503.119519	290160.318743	42.731930
3503.159962	290124.521369	42.736935
3503.133346	290086.621549	42.741940
3503.277179	290047.498742	42.746944
3503.018005	290009.304135	42.751949
3503.047803	289965.107784	42.756954
3503.070476	289927.302024	42.761959
3503.021840	289884.543371	42.766964
3503.241214	289837.542701	42.771968
3502.874941	289803.106705	42.776973
3503.175032	289754.464212	42.781978
3503.428949	289718.709760	42.786983
3503.260744	289676.707807	42.791988
3503.472705	289626.195162	42.796993
3503.019267	289593.198173	42.801997
3503.092437	289544.336268	42.807002
3503.002872	289512.708170	42.812007
3502.546895	289471.692750	42.817012
3502.926115	289428.078063	42.822017
3503.097378	289400.456892	42.827021
3503.173600	289353.350861	42.832026
3502.719460	289318.266409	42.837031
3502.636763	289277.269147	42.842036
3503.004720	289233.477886	42.847041
3502.607875	289208.668883	42.852045
3502.936755	289174.048004	42.857050
3502.702245	289128.441183	42.862055
3503.085120	289092.360836	42.867060
3503.297427	289044.647901	42.872065
3503.120660	289011.913038	42.877069
3503.252431	288975.082545	42.882074
3503.037517	288932.196393	42.887079
3502.916383	288882.498696	42.892084
3503.019589	288841.675881	42.897089
3502.660711	288815.155223	42.902093
3502.999877	288768.695177	42.907098
3503.115211	288735.049191	42.912103
3502.874242	288686.642827	42.917108
3503.297281	288654.934541	42.922113
3503.286749	288626.781281	42.927117
3503.351280	288578.607321	42.932122
3502.882546	288533.418380	42.937127
3502.629344	288492.014387	42.942132
3503.053227	288456.869206	42.947137
3502.920510	288412.875276	42.952141
3503.043038	288379.686210	42.957146
3503.100935	288341.288530	42.962151
3502.704970	288305.990821	42.967156
3503.083553	288263.648293	42.972161
3502.909222	288226.915924	42.977165
3503.058197	288177.506596	42.982170
3502.997972	288136.097804	42.987175
3502.754831	288101.641739	42.992180
3502.842647	288054.049278	42.997185
3503.154099	288030.707935	43.002189
3503.132341	287987.460162	43.007194
3503.119866	287946.603874	43.012199
3502.776510	287907.377384	43.017204
3502.902803	287863.164580	43.022209
3502.797405	287825.657548	43.027213
3502.750310	287782.439040	43.032218
3502.560465	287754.033280	43.037223
3502.547239	287720.788633	43.042228
3503.065407	287679.569577	43.047233
3502.588024	287649.935661	43.052237
3502.668417	287602.344028	43.057242
3502.521988	287567.439862	43.062247
3502.436520	287544.211027	43.067252
3502.867292	287504.889291	43.072257
3502.407181	287480.878647	43.077261
3502.541651	287438.649946	43.082266
3502.846924	287400.595080	43.087271
3502.951134	287377.845815	43.092276
3503.024518	287336.415729	43.097281
3502.552951	287306.500725	43.102285
3502.887982	287263.069669	43.107290
3502.691605	287232.882693	43.112295
3502.563874	287198.128166	43.117300
3502.986703	287151.119354	43.122305
3502.505453	287123.980620	43.127309
3502.403739	287094.822601	43.132314
3502.514593	287052.673702	43.137319
3502.269532	287019.439323	43.142324
3502.757128	286982.603256	43.147329
3502.465468	286964.854183	43.152333
3502.541531	286931.162471	43.157338
3502.683106	286895.678528	43.162343
3502.697099	286857.770509	43.167348
3502.997258	286815.973863	43.172353
3502.637071	286783.342803	43.177357
3502.422476	286751.172762	43.182362
3502.375432	286716.583630	43.187367
3502.650981	286688.206823	43.192372
3502.898990	286646.800049	43.197377
3502.418175	286624.905290	43.202381
3502.459796	286582.385005	43.207386
3502.926724	286550.210645	43.212391
3502.659944	286513.262593	43.217396
3502.633932	286475.029634	43.222401
3502.684768	286451.626462	43.227405
3502.496226	286412.756862	43.232410
3502.293017	286382.265074	43.237415
3502.394172	286348.161843	43.242420
3502.811463	286309.605230	43.247425
3502.597142	286289.985535	43.252429
3502.609937	286248.360543	43.257434
3502.606868	286208.774607	43.262439
3502.501006	286185.293896	43.267444
3502.720088	286142.363854	43.272449
3502.544932	286113.395040	43.277453
3502.425664	286078.307665	43.282458
3502.749475	286056.440256	43.287463
3502.696788	286023.531856	43.292468
3502.862657	285981.373725	43.297473
3502.667947	285950.473094	43.302477
3502.566090	285911.997041	43.307482
3502.737776	285884.399792	43.312487
3502.717689	285850.035141	43.317492
3502.982051	285803.864697	43.322497
3502.633109	285767.081769	43.327501
3502.857240	285733.264586	43.332506
3502.578952	285695.757805	43.337511
3502.814711	285669.245186	43.342516
3503.118025	285623.755921	43.347521
3502.831976	285593.913116	43.352525
3502.890474	285557.804952	43.357530
3502.772161	285518.185630	43.362535
3502.619503	285480.022733	43.367540
3502.613905	285437.636368	43.372545
3502.464234	285412.711105	43.377549
3502.536620	285375.022289	43.382554
3502.711290	285345.820504	43.387559
3502.437779	285310.985858	43.392564
3502.607671	285275.623950	43.397569
3502.429833	285246.782475	43.402573
3502.422749	285208.240361	43.407578
3502.450726	285181.658054	43.412583
3502.647503	285153.649277	43.417588
3502.564124	285123.621979	43.422593
3502.090217	285094.902886	43.427597
3502.245556	285050.225468	43.432602
3502.479836	285023.178210	43.437607
3502.186778	284996.874912	43.442612
3502.909795	284958.091754	43.447617
3502.696740	284934.194505	43.452621
3502.414091	284897.553543	43.457626
3502.509917	284854.896454	43.462631
3502.114000	284835.228225	43.467636
3502.479533	284792.783709	43.472641
3502.474809	284765.238919	43.477645
3502.182162	284732.876404	43.482650
3502.383707	284705.808657	43.487655
3502.069982	284678.057334	43.492660
3502.268255	284640.068486	43.497665
3502.397658	284625.435559	43.502669
3502.395400	284600.818019	43.507674
3502.649729	284559.867246	43.512679
3501.950299	284532.506843	43.517684
3502.568100	284502.446538	43.522689
3502.267772	284478.460880	43.527693
3502.481510	284440.978682	43.532698
3502.336784	284404.417830	43.537703
3502.191343	284380.637160	43.542708
3502.544467	284355.149565	43.547713
3502.731433	284330.171525	43.552717
3502.736003	284292.772714	43.557722
3502.672321	284259.152345	43.562727
3502.145778	284222.192562	43.567732
3502.496635	284189.016820	43.572737
3502.255506	284155.780433	43.577741
3502.451269	284119.319197	43.582746
3502.741577	284091.982814	43.587751
3502.205347	284063.043865	43.592756
3502.205725	284033.155813	43.597761
3502.450458	283997.425190	43.602765
3502.474731	283975.629193	43.607770
3502.592498	283951.960169	43.612775
3502.554726	283925.896783	43.617780
3502.498908	283884.408331	43.622785
3502.372396	283848.964528	43.627789
3502.005298	283820.559248	43.632794
3502.257437	283790.097286	43.637799
3502.320069	283762.312492	43.642804
3502.323400	283726.517461	43.647809
3502.298065	283701.775903	43.652813
3502.707055	283662.353511	43.657818
3502.903061	283640.250642	43.662823
3502.621026	283605.874722	43.667828
3502.997845	283560.067163	43.672833
3502.412909	283522.886970	43.677837
3502.501368	283498.458595	43.682842
3502.641924	283465.009734	43.687847
3502.739528	283429.276259	43.692852
3502.604524	283404.704415	43.697857
3502.681551	283376.942687	43.702861
3502.797787	283337.998469	43.707866
3502.730673	283294.652941	43.712871
3502.300087	283266.613739	43.717876
3502.400454	283222.732930	43.722881
3502.318940	283204.695595	43.727885
3502.736412	283172.756489	43.732890
3502.389618	283129.938099	43.737895
3502.246950	283114.583431	43.742900
3502.323763	283073.277534	43.747905
3502.181751	283043.513056	43.752909
3502.467084	283018.264657	43.757914
3502.415591	282984.718161	43.762919
3502.087485	282954.295215	43.767924
3502.606225	282918.903291	43.772929
3502.210851	282902.518629	43.777933
3502.049161	282865.832324	43.782938
3502.206303	282842.869652	43.787943
3502.057002	282817.205097	43.792948
3502.435559	282778.397965	43.797953
3502.521493	282758.144993	43.802957
3502.646656	282719.682768	43.807962
3502.505634	282693.176735	43.812967
3502.218377	282659.641315	43.817972
3502.431404	282627.071847	43.822977
3502.323193	282609.165811	43.827981
3502.207987	282574.687054	43.832986
3502.358495	282544.036702	43.837991
3502.081857	282512.841790	43.842996
3502.567071	282475.519979	43.848001
3501.969249	282451.019827	43.853005
3501.955306	282432.309847	43.858010
3502.204675	282405.641122	43.863015
3502.115077	282371.463792	43.868020
3502.552480	282339.826723	43.873025
3502.235734	282319.865421	43.878029
3502.020340	282291.919646	43.883034
3502.693372	282264.904891	43.888039
3502.313074	282236.704705	43.893044
3502.221693	282199.981660	43.898049
3502.167308	282168.726554	43.903053
3502.378421	282139.110424	43.908058
3502.305447	282100.500487	43.913063
3501.764673	282088.517241	43.918068
3502.222078	282058.786374	43.923073
3501.912589	282033.044630	43.928077
3502.067624	282003.819059	43.933082
3502.003390	281975.671424	43.938087
3501.903483	281965.605371	43.943092
3501.992169	281934.607952	43.948097
3502.116227	281916.691060	43.953101
3502.498879	281892.394573	43.958106
3502.309453	281856.170336	43.963111
3502.015620	281827.931076	43.968116
3502.237986	281793.272121	43.973121
3502.213353	281773.239752	43.978125
3502.411920	281740.773973	43.983130
3502.605609	281714.571926	43.988135
3502.163151	281678.845243	43.993140
3502.311863	281654.406866	43.998145
3501.849248	281619.701664	44.003149
3502.336334	281590.857064	44.008154
3502.204486	281565.214808	44.013159
3502.111046	281550.946899	44.018164
3502.198562	281519.669432	44.023169
3502.557753	281483.792448	44.028173
3502.286918	281461.074153	44.033178
3502.459301	281434.697105	44.038183
3502.407623	281399.775095	44.043188
3502.460909	281360.992362	44.048193
3502.222065	281332.795273	44.053197
3502.256155	281297.477977	44.058202
3502.297530	281272.037797	44.063207
3501.924402	281253.077895	44.068212
3502.641405	281232.420781	44.073217
3502.350114	281206.955968	44.078221
3502.114348	281169.109195	44.083226
3502.017334	281141.908342	44.088231
3501.883878	281118.608454	44.093236
3502.006163	281094.632274	44.098241
3502.441251	281062.383984	44.103245
3502.332306	281029.354714	44.108250
3502.113025	281002.198295	44.113255
3501.894910	280974.456115	44.118260
3502.216051	280944.822380	44.123265
3502.167553	280923.622353	44.128269
3502.123901	280885.745540	44.133274
3502.330289	280868.197474	44.138279
3502.139072	280845.161084	44.143284
3502.149899	280808.345057	44.148289
3502.051813	280788.527527	44.153293
3501.914932	280757.233737	44.158298
3502.556750	280737.632031	44.163303
3502.447887	280711.425789	44.168308
3502.170429	280668.773375	44.173313
3502.262873	280642.484863	44.178317
3502.129692	280614.271057	44.183322
3502.309025	280582.724310	44.188327
3502.358010	280573.500526	44.193332
3502.276103	280538.786491	44.198337
3502.395541	280512.646491	44.203341
3502.427506	280487.691241	44.208346
3502.385022	280452.716434	44.213351
3501.914845	280420.914253	44.218356
3501.940037	280385.928884	44.223361
3502.364150	280375.628311	44.228365
3502.295580	280339.562740	44.233370
3502.358535	280309.383355	44.238375
3502.235684	280288.449315	44.243380
3502.279008	280250.380426	44.248385
3502.040387	280228.726051	44.253389
3501.965382	280207.275347	44.258394
3502.543354	280167.799307	44.263399
3502.072146	280144.169775	44.268404
3502.329311	280115.003943	44.273409
3502.014126	280090.178961	44.278413
3501.974375	280057.596770	44.283418
3502.477451	280026.457688	44.288423
3502.157695	280004.663114	44.293428
3502.273795	279972.973190	44.298433
3502.036498	279954.781076	44.303437
3502.111128	279924.828858	44.308442
3502.255841	279893.541807	44.313447
3501.761362	279878.037527	44.318452
3502.164318	279851.547659	44.323457
3502.385966	279826.180773	44.328461
3501.749203	279799.241641	44.333466
3502.147867	279775.222030	44.338471
3502.154671	279740.341061	44.343476
3502.239971	279707.382819	44.348481
3501.933235	279697.094043	44.353485
3501.597645	279663.310179	44.358490
3501.977923	279634.150464	44.363495
3501.754772	279617.356367	44.368500
3502.027676	279596.004111	44.373505
3502.313737	279576.279243	44.378509
3502.277630	279546.013127	44.383514
3502.234434	279521.196553	44.388519
3502.213809	279489.655003	44.393524
3502.335912	279450.325908	44.398529
3502.368290	279428.909193	44.403533
3501.711877	279398.484945	44.408538
3502.031268	279374.095642	44.413543
3502.202658	279349.703901	44.418548
3502.305624	279321.580164	44.423553
3502.375733	279294.556314	44.428557
3502.042575	279276.862696	44.433562
3502.083454	279237.571591	44.438567
3502.021767	279213.063316	44.443572
3501.865908	279184.801583	44.448577
3502.010261	279168.204800	44.453581
3502.027931	279136.911747	44.458586
3502.429236	279105.864505	44.463591
3501.835763	279093.634372	44.468596
3501.700398	279068.042727	44.473601
3502.069426	279044.791303	44.478605
3501.992487	279012.367212	44.483610
3502.344090	278995.152556	44.488615
3502.191695	278972.185933	44.493620
3501.873043	278926.356415	44.498625
3501.734169	278914.768400	44.503629
3501.741940	278892.795238	44.508634
3502.175144	278867.802477	44.513639
3501.840199	278840.586896	44.518644
3501.985435	278814.365915	44.523649
3501.655748	278794.100156	44.528653
3501.707630	278772.094636	44.533658
3501.843351	278751.807363	44.538663
3501.841557	278733.247325	44.543668
3501.777429	278699.649934	44.548673
3502.259714	278686.513986	44.553677
3502.035013	278658.848359	44.558682
3502.344804	278638.814033	44.563687
3502.292190	278610.128658	44.568692
3502.399931	278578.566757	44.573697
3502.057194	278545.980148	44.578701
3502.198578	278525.717396	44.583706
3502.319521	278491.327303	44.588711
3501.882577	278473.395046	44.593716
3502.180730	278440.835964	44.598721
3502.129703	278416.834984	44.603725
3502.373617	278394.086582	44.608730
3502.425100	278359.783622	44.613735
3502.150630	278330.368853	44.618740
3502.077020	278310.495946	44.623745
3502.116519	278284.444002	44.628749
3502.229253	278252.499285	44.633754
3502.170114	278220.275775	44.638759
3502.046701	278190.862907	44.643764
3502.175961	278170.398265	44.648769
3501.965434	278147.567744	44.653773
3502.315742	278125.082773	44.658778
3502.435000	278087.077371	44.663783
3502.109371	278070.044278	44.668788
3502.255617	278027.833661	44.673793
3502.132952	278010.896273	44.678797
3501.778682	277977.802009	44.683802
3502.157333	277952.766522	44.688807
3501.654043	277924.329247	44.693812
3501.855608	277902.452951	44.698817
3501.728376	277880.678735	44.703821
3501.522236	277865.663850	44.708826
3502.007114	277829.001761	44.713831
3501.952937	277815.669080	44.718836
3502.025766	277797.173588	44.723841
3501.626937	277770.247639	44.728845
3501.632243	277754.079562	44.733850
3502.246406	277731.273351	44.738855
3501.751417	277709.810922	44.743860
3501.984830	277694.091088	44.748865
3501.963818	277658.958899	44.753869
3501.735345	277640.586639	44.758874
3502.150508	277619.364464	44.763879
3501.821553	277602.000797	44.768884
3501.953542	277568.219636	44.773889
3502.039188	277546.794111	44.778893
3501.805115	277522.159363	44.783898
3501.662961	277494.429556	44.788903
3501.560436	277484.363314	44.793908
3501.877059	277449.789549	44.798913
3501.721994	277435.657759	44.803917
3501.738778	277413.122642	44.808922
3501.759451	277387.175172	44.813927
3502.088177	277365.940919	44.818932
3502.459648	277340.422600	44.823937
3501.864250	277325.060813	44.828941
3502.237238	277285.156904	44.833946
3502.240581	277260.688816	44.838951
3501.886495	277240.324607	44.843956
3502.366205	277205.267062	44.848961
3501.927168	277187.156610	44.853965
3501.753589	277155.917983	44.858970
3501.935996	277137.430746	44.863975
3501.921368	277117.471976	44.868980
3501.597828	277090.152166	44.873985
3501.711618	277073.559695	44.878989
3501.555467	277054.615905	44.883994
3501.884026	277036.335049	44.888999
3501.854930	277023.482088	44.894004
3501.963233	276994.287323	44.899009
3501.673488	276971.850702	44.904013
3501.593254	276943.398163	44.909018
3501.843372	276930.068902	44.914023
3501.549500	276912.394093	44.919028
3501.664375	276879.659199	44.924033
3501.501135	276863.542628	44.929037
3501.516188	276844.470304	44.934042
3501.779685	276821.845705	44.939047
3501.981547	276806.359754	44.944052
3501.919899	276781.774327	44.949057
3501.904910	276761.662759	44.954061
3502.066955	276741.116261	44.959066
3501.873206	276710.924498	44.964071
3501.582455	276699.232483	44.969076
3501.555452	276674.336100	44.974081
3501.823500	276661.818756	44.979085
3501.893017	276631.611455	44.984090
3501.827476	276609.572680	44.989095
3501.789276	276587.860638	44.994100
3501.717610	276571.958907	44.999105
3501.791015	276547.072321	45.004109
3501.635125	276517.129203	45.009114
3501.873622	276498.225714	45.014119
3501.704839	276480.098507	45.019124
3501.827280	276456.681002	45.024129
3501.835440	276438.297102	45.029133
3501.570669	276427.033843	45.034138
3502.116068	276408.158957	45.039143
3501.768765	276382.090196	45.044148
3502.220902	276364.630172	45.049153
3501.780819	276332.898012	45.054157
3502.017543	276307.935015	45.059162
3502.112093	276275.686799	45.064167
3501.954279	276258.321668	45.069172
3502.327699	276232.395316	45.074177
3501.812130	276205.817998	45.079181
3501.998649	276193.949796	45.084186
3502.280942	276164.294816	45.089191
3502.181969	276147.124194	45.094196
3501.983869	276114.284925	45.099201
3502.220476	276079.952171	45.104205
3501.998668	276052.616177	45.109210
3502.221122	276023.887060	45.114215
3501.946185	276001.524247	45.119220
3502.229770	275971.028776	45.124225
3502.133657	275949.885720	45.129229
3502.311589	275929.871230	45.134234
3502.086869	275894.388048	45.139239
3501.940548	275876.740974	45.144244
3501.979400	275846.741842	45.149249
3502.099855	275827.296418	45.154253
3502.156677	275798.032848	45.159258
3502.144585	275767.761541	45.164263
3502.009486	275746.879112	45.169268
3501.792339	275725.067378	45.174273
3501.700399	275700.817333	45.179277
3501.425484	275683.648530	45.184282
3502.036391	275656.870278	45.189287
3501.735323	275631.761609	45.194292
3501.798063	275614.234713	45.199297
3502.123571	275585.463944	45.204301
3501.842542	275570.918586	45.209306
3502.095515	275544.017766	45.214311
3501.730717	275528.492443	45.219316
3502.016790	275506.118578	45.224321
3501.845138	275471.900022	45.229325
3501.687467	275457.742828	45.234330
3502.224228	275428.200751	45.239335
3501.923278	275409.839258	45.244340
3501.721793	275381.150424	45.249345
3502.025034	275358.493772	45.254349
3501.579857	275327.347625	45.259354
3501.976755	275323.441438	45.264359
3502.045029	275296.594740	45.269364
3501.866529	275258.608872	45.274369
3502.319509	275240.333712	45.279373
3502.267142	275212.028997	45.284378
3502.214690	275184.768205	45.289383
3502.181245	275157.911830	45.294388
3501.736445	275127.758545	45.299393
3501.876791	275105.203556	45.304397
3501.712704	275074.191802	45.309402
3502.261854	275053.049950	45.314407
3501.670963	275036.541258	45.319412
3501.893091	275021.561044	45.324417
3502.118321	274993.391287	45.329421
3501.889624	274976.342452	45.334426
3502.050006	274948.641079	45.339431
3501.734085	274930.536424	45.344436
3501.598433	274900.284026	45.349441
3502.133599	274885.280536	45.354445
3501.907801	274861.560304	45.359450
3502.068103	274818.301896	45.364455
3501.640767	274811.723175	45.369460
3501.740641	274787.162935	45.374465
3501.890310	274761.678323	45.379469
3501.872301	274752.846206	45.384474
3502.120136	274719.631446	45.389479
3502.245751	274690.738703	45.394484
3501.894219	274678.368393	45.399489
3501.955012	274649.893108	45.404493
3502.000050	274618.874103	45.409498
3502.234660	274592.026755	45.414503
3502.090516	274570.025125	45.419508
3501.882383	274545.028972	45.424513
3501.966066	274524.035804	45.429517
3502.010912	274502.132054	45.434522
3502.056872	274473.633555	45.439527
3501.916962	274453.642706	45.444532
3501.785562	274423.618628	45.449537
3501.990054	274389.773941	45.454541
3501.634963	274382.776557	45.459546
3501.716856	274354.883507	45.464551
3501.544612	274349.792757	45.469556
3501.401560	274324.735487	45.474561
3501.812542	274299.642920	45.479565
3501.329839	274285.052333	45.484570
3501.575809	274257.311950	45.489575
3501.731952	274244.200571	45.494580
3501.758911	274219.651511	45.499585
3501.542318	274201.098392	45.504589
3501.186264	274190.791115	45.509594
3501.632859	274169.563152	45.514599
3501.475493	274157.417169	45.519604
3501.916393	274140.594968	45.524609
3501.826802	274109.902267	45.529613
3501.614804	274099.623486	45.534618
3501.692801	274064.678034	45.539623
3501.274705	274056.213644	45.544628
3501.382580	274026.126728	45.549633
3501.817021	274021.348938	45.554637
3501.538830	274000.259181	45.559642
3501.807341	273982.445303	45.564647
3501.590281	273971.810828	45.569652
3501.434293	273939.447917	45.574657
3501.714496	273920.079036	45.579661
3501.251248	273908.489852	45.584666
3501.494381	273896.026890	45.589671
3501.804947	273877.926365	45.594676
3501.459746	273850.277843	45.599681
3501.743741	273834.676705	45.604685
3501.131299	273810.634415	45.609690
3501.285564	273796.912175	45.614695
3501.762660	273794.139222	45.619700
3501.807069	273772.235351	45.624705
3501.870606	273748.749861	45.629709
3501.733850	273721.578097	45.634714
3501.671862	273707.278408	45.639719
3501.633635	273682.128251	45.644724
3501.855098	273664.983638	45.649729
3501.596751	273647.862761	45.654733
3501.336172	273634.332359	45.659738
3501.782149	273618.705975	45.664743
3501.609017	273595.308196	45.669748
3501.452860	273574.632195	45.674753
3501.843436	273549.313424	45.679757
3501.262996	273534.610607	45.684762
3501.665003	273518.736428	45.689767
3501.606308	273490.864971	45.694772
3501.723442	273481.553376	45.699777
3501.755859	273460.058682	45.704781
3501.532667	273453.830017	45.709786
3501.351067	273429.033101	45.714791
3501.399661	273412.730121	45.719796
3501.728707	273397.834829	45.724801
3501.763838	273374.404580	45.729805
3501.952174	273364.139799	45.734810
3502.156534	273323.572741	45.739815
3502.126383	273304.099243	45.744820
3502.061889	273268.615474	45.749825
3501.777764	273190.415104	45.754829
3501.285113	273083.958749	45.759834
3501.125728	272933.528254	45.764839
3500.637362	272739.048209	45.769844
3499.797190	272504.264822	45.774849
3499.512373	272224.886245	45.779853
3498.416023	271906.115395	45.784858
3497.416709	271551.324297	45.789863
3496.255862	271160.756468	45.794868
3495.215503	270735.284226	45.799873
3493.901521	270266.845767	45.804877
3492.320609	269782.226511	45.809882
3490.639832	269257.261158	45.814887
3489.258065	268707.063128	45.819892
3487.407709	268117.950270	45.824897
3485.867017	267497.134335	45.829901
3483.858483	266868.238847	45.834906
3481.830407	266187.676042	45.839911
3479.290302	265511.491764	45.844916
3477.726106	264783.305837	45.849921
3475.843120	264040.573293	45.854925
3472.431542	263286.385159	45.859930
3470.242306	262505.874643	45.864935
3467.920799	261701.874999	45.869940
3465.370201	260879.468493	45.874945
3462.565097	260037.996721	45.879949
3459.753969	259196.443538	45.884954
3457.059856	258319.112422	45.889959
3454.197482	257443.176505	45.894964
3451.867343	256532.925358	45.899969
3448.733714	255614.822046	45.904973
3445.393261	254702.831228	45.909978
3442.710717	253753.932867	45.914983
3439.560287	252809.532353	45.919988
3436.395504	251856.418462	45.924993
3433.495805	250875.141833	45.929997
3430.241801	249904.305043	45.935002
3427.076322	248911.903481	45.940007
3423.381944	247916.955473	45.945012
3419.951030	246915.415892	45.950017
3416.800971	245910.007229	45.955021
3413.447228	244910.610225	45.960026
3410.005961	243881.297198	45.965031
3406.737458	242867.029720	45.970036
3402.804642	241854.109241	45.975041
3399.954832	240818.705895	45.980045
3396.315049	239793.379678	45.985050
3392.715011	238754.163297	45.990055
3389.073355	237725.901448	45.995060
3385.644080	236682.296754	46.000065
3382.080141	235643.752904	46.005069
3378.542802	234601.891342	46.010074
3374.880626	233545.453176	46.015079
3371.083975	232512.923646	46.020084
3367.676953	231475.263383	46.025089
3364.297780	230427.409665	46.030093
3360.633382	229395.211576	46.035098
3356.824187	228339.527124	46.040103
3353.215527	227295.628392	46.045108
3349.361538	226245.221860	46.050113
3345.632349	225196.655003	46.055117
3342.168890	224167.301542	46.060122
3338.707385	223120.221716	46.065127
3334.904412	222080.963774	46.070132
3330.953155	221040.074378	46.075137
3327.369496	219999.587457	46.080141
3323.368777	218961.128054	46.085146
3320.322143	217930.366377	46.090151
3316.202476	216892.846177	46.095156
3312.176920	215863.565534	46.100161
3308.828389	214827.254601	46.105165
3304.686111	213814.552120	46.110170
3301.346131	212772.770031	46.115175
3297.419746	211753.418471	46.120180
3293.670913	210731.521461	46.125185
3289.915647	209721.777644	46.130189
3285.981468	208713.288129	46.135194
3282.275683	207693.001057	46.140199
3278.621555	206695.147794	46.145204
3274.906293	205694.125198	46.150209
3270.848611	204686.488258	46.155213
3266.812950	203692.554663	46.160218
3263.384641	202687.606353	46.165223
3259.896461	201700.500141	46.170228
3255.970576	200715.123130	46.175233
3252.123673	199735.902774	46.180237
3248.354824	198748.985390	46.185242
3245.065521	197757.135681	46.190247
3241.462593	196789.229048	46.195252
3237.298273	195815.890222	46.200257
3233.414246	194833.245049	46.205261
3229.389164	193866.061467	46.210266
3225.534130	192894.656870	46.215271
3221.882592	191933.210669	46.220276
3218.514896	190977.075655	46.225281
3214.439894	190024.954642	46.230285
3210.502458	189089.092208	46.235290
3206.742418	188132.532703	46.240295
3203.021339	187193.240449	46.245300
3198.893178	186263.568946	46.250305
3195.852137	185322.812566	46.255309
3191.639417	184399.562618	46.260314
3188.031414	183486.692696	46.265319
3184.297032	182557.350854	46.270324
3180.239684	181641.207314	46.275329
3176.506509	180723.723784	46.280333
3172.565628	179813.844215	46.285338
3168.710093	178918.244992	46.290343
3165.183651	178020.999643	46.295348
3161.278477	177123.007857	46.300353
3157.362093	176230.170622	46.305357
3153.474241	175358.013080	46.310362
3149.793001	174467.640957	46.315367
3146.233663	173593.350918	46.320372
3141.979922	172724.805427	46.325377
3137.961846	171860.128442	46.330381
3134.215704	171009.549164	46.335386
3130.991243	170152.889966	46.340391
3126.743261	169297.061969	46.345396
3122.689320	168444.650845	46.350401
3119.193849	167608.405566	46.355405
3115.159897	166778.223998	46.360410
3111.412752	165944.532740	46.365415
3107.779486	165125.497537	46.370420
3103.989584	164298.324866	46.375425
3100.040078	163475.069521	46.380429
3095.873509	162677.429536	46.385434
3091.915663	161869.457067	46.390439
3088.448679	161078.499439	46.395444
3084.593969	160287.637512	46.400449
3080.716766	159498.354623	46.405453
3076.733889	158728.024147	46.410458
3073.225216	157943.476772	46.415463
3069.094418	157186.145407	46.420468
3065.030695	156424.664219	46.425473
3061.233280	155662.196923	46.430477
3057.219448	154909.305606	46.435482
3054.000138	154167.945291	46.440487
3049.816342	153429.468154	46.445492
3045.750381	152704.663045	46.450497
3042.372936	151974.198906	46.455501
3037.807569	151265.881449	46.460506
3034.098080	150547.323007	46.465511
3030.031236	149844.125823	46.470516
3026.023714	149154.862925	46.475521
3022.020923	148473.726915	46.480525
3018.304876	147802.009807	46.485530
3014.100958	147127.132389	46.490535
3010.006989	146452.908329	46.495540
3005.784756	145808.055960	46.500545
3002.281456	145149.586528	46.505549
2998.173295	144526.898619	46.510554
2994.275734	143882.083894	46.515559
2990.370576	143274.394435	46.520564
2986.357416	142655.557770	46.525569
2982.868297	142040.858881	46.530573
2978.936210	141442.204635	46.535578
2975.346933	140840.858006	46.540583
2971.576658	140255.909050	46.545588
2967.538660	139658.794857	46.550593
2963.895949	139075.049275	46.555597
2959.503515	138505.282610	46.560602
2956.034151	137938.267267	46.565607
2952.343816	137377.056472	46.570612
2948.260428	136821.893118	46.575617
2944.860157	136258.157290	46.580621
2941.154050	135718.469557	46.585626
2937.382794	135171.648770	46.590631
2933.900794	134621.125795	46.595636
2930.373193	134094.889222	46.600641
2926.624244	133553.504092	46.605645
2922.644539	133014.069676	46.610650
2919.277543	132472.625669	46.615655
2915.869693	131875.452101	46.620660
2911.910733	131341.110733	46.625665
2908.248694	130816.410076	46.630669
2904.977394	130292.151125	46.635674
2901.176397	129775.753079	46.640679
2897.528390	129262.568399	46.645684
2893.858230	128747.688943	46.650689
2890.091264	128230.693953	46.655693
2886.636288	127721.848215	46.660698
2883.242932	127207.402579	46.665703
2879.906109	126702.748375	46.670708
2876.159642	126200.135573	46.675713
2872.710854	125676.801630	46.680717
2868.911112	125186.139977	46.685722
2865.516171	124678.098510	46.690727
2862.127340	124175.366099	46.695732
2858.365925	123671.998467	46.700737
2854.706372	123173.072689	46.705741
2851.077699	122671.706525	46.710746
2847.676232	122165.160652	46.715751
2844.433945	121671.097995	46.720756
2840.719353	121173.986573	46.725761
2837.458305	120672.423441	46.730765
2833.655170	120180.349151	46.735770
2830.033909	119676.260702	46.740775
2826.525084	119175.442323	46.745780
2822.885559	118677.690138	46.750785
2819.384240	118180.393474	46.755789
2815.856729	117690.355739	46.760794
2812.097963	117184.350706	46.765799
2808.391941	116700.050513	46.770804
2804.463785	116216.376105	46.775809
2801.226586	115737.953770	46.780813
2797.712955	115252.142068	46.785818
2794.025629	114762.320328	46.790823
2790.683799	114280.334775	46.795828
2786.854028	113798.113645	46.800833
2783.664570	113317.897220	46.805837
2779.662020	112848.277873	46.810842
2776.174418	112367.739043	46.815847
2772.493009	111890.389964	46.820852
2769.074998	111426.661289	46.825857
2765.480990	110954.867229	46.830861
2761.800133	110488.127644	46.835866
2757.722820	110009.721223	46.840871
2754.372396	109545.307458	46.845876
2750.276588	109088.542140	46.850881
2747.189185	108633.342158	46.855885
2743.385833	108177.407790	46.860890
2739.680532	107722.112530	46.865895
2735.971665	107281.049307	46.870900
2731.915521	106839.664423	46.875905
2728.270156	106400.623947	46.880909
2724.737935	105963.325802	46.885914
2720.851685	105530.537590	46.890919
2716.800079	105103.310306	46.895924
2713.001146	104690.159095	46.900929
2709.755576	104266.325438	46.905933
2705.741610	103851.247750	46.910938
2702.337466	103441.266507	46.915943
2698.635979	103027.726656	46.920948
2694.950406	102626.849553	46.925953
2691.356552	102218.349309	46.930957
2687.589827	101819.159773	46.935962
2684.216115	101422.862760	46.940967
2680.471661	101028.102642	46.945972
2676.783749	100636.058479	46.950977
2673.801079	100239.829398	46.955981
2669.594936	99841.850962	46.960986
2665.999089	99453.912068	46.965991
2662.629489	99060.566521	46.970996
2658.947174	98675.383035	46.976001
2655.748050	98286.532294	46.981005
2652.425395	97898.773081	46.986010
2648.683090	97515.697238	46.991015
2645.239018	97126.682763	46.996020
2641.434460	96741.440087	47.001025
2638.346058	96343.865173	47.006029
2634.724610	95964.792527	47.011034
2631.323481	95578.192401	47.016039
2627.595945	95190.720182	47.021044
2623.761027	94807.755357	47.026049
2620.880051	94415.802291	47.031053
2617.545245	94034.395782	47.036058
2613.752435	93645.847510	47.041063
2610.292978	93264.482650	47.046068
2606.959639	92867.460590	47.051073
2603.829884	92475.443914	47.056077
2600.364767	92090.968704	47.061082
2596.401527	91708.392913	47.066087
2593.476076	91303.627642	47.071092
2589.876495	90905.935692	47.076097
2586.450830	90504.765896	47.081101
2582.663391	90106.669048	47.086106
2579.170208	89713.880793	47.091111
2576.004655	89315.253013	47.096116
2572.633472	88922.075047	47.101121
2568.917560	88519.655761	47.106125
2565.278509	88115.756212	47.111130
2562.134178	87716.854429	47.116135
2558.587246	87318.439965	47.121140
2554.816376	86920.434196	47.126145
2551.448956	86521.329311	47.131149
2547.915853	86116.500707	47.136154
2544.711104	85718.194586	47.141159
2541.064766	85308.910379	47.146164
2537.221119	84911.134022	47.151169
2534.190617	84501.867057	47.156173
2530.321072	84102.276627	47.161178
2527.397919	83699.254401	47.166183
2523.784367	83291.086311	47.171188
2519.769790	82888.258102	47.176193
2516.852499	82478.176843	47.181197
2513.121754	82074.515769	47.186202
2509.244751	81669.816248	47.191207
2505.901639	81260.161907	47.196212
2502.293452	80865.517497	47.201217
2499.132785	80463.962842	47.206221
2495.236723	80051.884618	47.211226
2492.107944	79650.209709	47.216231
2488.646293	79233.211448	47.221236
2485.137229	78830.362899	47.226241
2481.894371	78417.381771	47.231245
2478.323965	78013.221143	47.236250
2474.627894	77604.234514	47.241255
2471.478051	77194.965789	47.246260
2467.829355	76789.654308	47.251265
2464.600214	76366.326166	47.256269
2460.668654	75957.121512	47.261274
2457.129079	75540.725022	47.266279
2453.843286	75130.289454	47.271284
2450.057451	74724.547680	47.276289
2446.683734	74302.569700	47.281293
2443.204279	73895.002283	47.286298
2439.611001	73470.252536	47.291303
2436.183368	73050.499556	47.296308
2432.638717	72659.913234	47.301313
2429.048344	72236.693832	47.306317
2425.474839	71818.087804	47.311322
2421.831586	71412.298225	47.316327
2418.660913	70992.563375	47.321332
2414.732917	70598.055004	47.326337
2411.570500	70178.541435	47.331341
2408.004324	69770.238690	47.336346
2404.473311	69353.404936	47.341351
2400.977371	68936.896183	47.346356
2397.260980	68521.114035	47.351361
2394.164963	68111.799406	47.356365
2390.562383	67698.786857	47.361370
2387.061742	67288.710419	47.366375
2383.702920	66870.404735	47.371380
2380.053930	66455.946856	47.376385
2376.593428	66040.653937	47.381389
2373.269267	65626.330427	47.386394
2369.734478	65190.529641	47.391399
2365.960495	64778.244968	47.396404
2362.872669	64374.396905	47.401409
2359.198904	63952.101068	47.406413
2355.503208	63528.654320	47.411418
2352.136538	63105.436455	47.416423
2348.942484	62687.009578	47.421428
2344.678818	62274.671063	47.426433
2342.018106	61844.688399	47.431437
2338.341479	61433.249885	47.436442
2334.799992	61002.574924	47.441447
2331.430336	60589.528920	47.446452
2327.551797	60159.524077	47.451457
2324.038569	59737.839995	47.456461
2320.640443	59316.132603	47.461466
2317.092814	58895.788352	47.466471
2313.632485	58471.122910	47.471476
2309.984362	58050.631292	47.476481
2306.645094	57628.893347	47.481485
2303.181649	57210.836889	47.486490
2299.365044	56780.488995	47.491495
2296.490121	56364.424165	47.496500
2292.486591	55937.553104	47.501505
2289.431849	55502.890399	47.506509
2285.718419	55085.468369	47.511514
2282.132408	54665.927515	47.516519
2278.668140	54247.796283	47.521524
2275.088052	53821.011636	47.526529
2272.079674	53387.046739	47.531533
2268.321977	52962.056297	47.536538
2264.660865	52546.694837	47.541543
2260.982617	52109.330696	47.546548
2256.782565	51684.705130	47.551553
2253.860194	51260.250064	47.556557
2250.384725	50840.373613	47.561562
2246.588801	50424.125918	47.566567
2243.335457	49994.594861	47.571572
2239.720230	49576.926175	47.576577
2236.669984	49155.358729	47.581581
2232.372690	48731.462343	47.586586
2229.486114	48312.529907	47.591591
2226.053364	47885.761967	47.596596
2222.707572	47466.117413	47.601601
2219.032436	47032.382152	47.606605
2215.309393	46607.833490	47.611610
2211.869173	46180.895888	47.616615
2208.632175	45749.793454	47.621620
2205.035199	45329.466691	47.626625
2201.954796	44896.016153	47.631629
2198.080066	44464.035718	47.636634
2194.116196	44039.141935	47.641639
2191.064258	43606.809106	47.646644
2187.322248	43194.820634	47.651649
2183.923128	42761.733961	47.656653
2180.261774	42323.611119	47.661658
2176.722954	41908.622080	47.666663
2173.468859	41482.982155	47.671668
2169.916060	41051.094402	47.676673
2166.431743	40622.469874	47.681677
2163.174657	40198.827295	47.686682
2159.525587	39769.896454	47.691687
2155.749478	39338.857233	47.696692
2152.215924	38909.906399	47.701697
2148.818276	38481.202861	47.706701
2145.522658	38057.164357	47.711706
2141.675497	37624.801030	47.716711
2138.396070	37199.420251	47.721716
2134.894363	36776.371025	47.726721
2131.511755	36341.191011	47.731725
2127.891184	35910.678125	47.736730
2124.512764	35484.281963	47.741735
2121.177263	35050.224012	47.746740
2117.494089	34627.797245	47.751745
2114.135315	34195.002860	47.756749
2110.433831	33766.105473	47.761754
2106.605970	33326.905012	47.766759
2103.348960	32892.156723	47.771764
2099.456771	32462.662833	47.776769
2096.212978	32030.776195	47.781773
2092.829076	31603.464527	47.786778
2088.904595	31170.478481	47.791783
2085.717804	30741.144837	47.796788
2081.961817	30323.506166	47.801793
2078.606781	29891.865161	47.806797
2075.323835	29468.333544	47.811802
2071.665010	29040.597994	47.816807
2068.282976	28603.924949	47.821812
2064.525108	28182.065357	47.826817
2061.077606	27755.635488	47.831821
2057.312069	27322.084789	47.836826
2053.692494	26892.835684	47.841831
2050.489669	26467.281852	47.846836
2046.740502	26040.858908	47.851841
2043.082942	25615.159348	47.856845
2039.967954	25199.813118	47.861850
2036.387268	24766.700281	47.866855
2032.994693	24332.433453	47.871860
2028.851697	23906.364162	47.876865
2025.477361	23490.067387	47.881869
2022.055702	23064.081209	47.886874
2018.475333	22651.381722	47.891879
2015.439078	22229.775295	47.896884
2011.848159	21805.920305	47.901889
2008.095110	21375.346935	47.906893
2004.639675	20962.935613	47.911898
2000.877604	20538.558060	47.916903
1997.423239	20101.733075	47.921908
1993.504389	19682.643164	47.926913
1990.184587	19269.042870	47.931917
1986.829790	18864.013757	47.936922
1983.304857	18441.437274	47.941927
1980.011301	18022.070403	47.946932
1976.341714	17608.262176	47.951937
1972.753696	17187.448683	47.956941
1969.224062	16773.931029	47.961946
1965.621369	16358.907367	47.966951
1962.299991	15939.472877	47.971956
1958.847299	15521.078055	47.976961
1955.518347	15097.100448	47.981965
1951.860168	14681.786090	47.986970
1947.707818	14269.277405	47.991975
1944.608099	13850.376659	47.996980
1940.748826	13433.015397	48.001985
1937.522020	13015.071001	48.006989
1933.950840	12608.843000	48.011994
1930.228270	12201.836852	48.016999
1926.793106	11783.781172	48.022004
1923.581830	11372.078748	48.027009
1919.875459	10951.709537	48.032013
1916.035789	10552.028711	48.037018
1912.227173	10148.439091	48.042023
1909.095532	9740.406759	48.047028
1905.648321	9330.318041	48.052033
1902.056015	8925.958398	48.057037
1898.589814	8522.920480	48.062042
1894.944960	8116.067196	48.067047
1891.066180	7716.345803	48.072052
1886.882023	7323.314388	48.077057
1883.427474	6939.106020	48.082061
1879.667752	6547.743666	48.087066
1876.054447	6166.870763	48.092071
1872.452970	5782.836065	48.097076
1867.916261	5417.496650	48.102081
1864.122656	5045.570998	48.107085
1860.161982	4706.944389	48.112090
1854.894773	4392.688141	48.117095
1849.719847	4089.017442	48.122100
1844.722654	3802.563638	48.127105
1840.527562	3518.710852	48.132109
1835.751044	3276.354336	48.137114
1831.359346	3030.153604	48.142119
1827.676385	2799.056192	48.147124
1823.722101	2581.616155	48.152129
1819.792043	2380.827722	48.157133
1815.964133	2185.461531	48.162138
1812.197886	1984.683679	48.167143
1808.622384	1793.958937	48.172148
1805.009781	1613.920439	48.177153
1801.024630	1428.803482	48.182157
1797.197801	1254.936844	48.187162
1793.722241	1093.884767	48.192167
1790.034523	930.835967	48.197172
1786.464468	775.031344	48.202177
1783.563125	616.165850	48.207181
1779.641145	475.687157	48.212186
1776.070320	322.224658	48.217191
1772.619892	188.258621	48.222196
1768.179110	55.548705	48.227201
1761.535728	-3.498915	48.232205
1752.254371	48.179104	48.237210
1746.481793	66.876803	48.242215
1742.786991	69.464227	48.247220
1740.406079	70.338069	48.252225
1737.743284	64.143769	48.257229
1735.263099	67.614647	48.262234
1732.399364	70.439714	48.267239
1730.025297	62.188360	48.272244
1726.595539	67.170587	48.277249
1723.264273	62.681167	48.282253
1719.631396	69.903275	48.287258
1716.167325	78.070372	48.292263
1713.243102	65.206539	48.297268
1709.444665	71.103514	48.302273
1706.062739	64.182762	48.307277
1702.570611	65.729422	48.312282
1699.091609	67.970054	48.317287
1696.107686	68.529633	48.322292
1692.584445	72.485554	48.327297
1689.276722	73.048075	48.332301
1686.038758	68.771922	48.337306
1682.102138	73.788750	48.342311
1678.653188	71.557553	48.347316
1675.185987	71.758925	48.352321
1671.900103	74.624390	48.357325
1668.029891	71.101530	48.362330
1664.956573	75.670786	48.367335
1661.716609	63.166151	48.372340
1657.997662	67.703017	48.377345
1654.563840	64.131222	48.382349
1651.165191	65.172963	48.387354
1647.549559	62.031257	48.392359
1644.484552	61.394926	48.397364
1641.086651	71.218994	48.402369
1637.285481	63.129660	48.407373
1634.096055	60.722038	48.412378
1630.318474	68.004635	48.417383
1626.851898	57.306955	48.422388
1623.491906	62.395384	48.427393
1619.869195	71.773560	48.432397
1616.888070	65.533909	48.437402
1612.880583	68.676202	48.442407
1609.345270	61.076997	48.447412
1605.958556	62.208631	48.452417
1602.306805	59.771732	48.457421
1599.352505	63.531538	48.462426
1596.074584	71.017938	48.467431
1592.611165	65.957490	48.472436
1588.627110	66.419645	48.477441
1584.968635	58.573863	48.482445
1582.060388	64.569567	48.487450
1578.060143	67.539896	48.492455
1574.887206	68.128903	48.497460
1571.402316	66.925189	48.502465
1567.896754	57.018187	48.507469
1564.581465	56.762497	48.512474
1560.910438	64.484084	48.517479
1557.800379	58.761213	48.522484
1553.844476	56.140709	48.527489
1550.204768	50.898905	48.532493
1546.631038	60.854738	48.537498
1543.278058	60.984560	48.542503
1540.049069	55.821196	48.547508
1536.560240	64.093382	48.552513
1532.831580	62.674519	48.557517
1529.695467	62.333997	48.562522
1526.163295	68.135754	48.567527
1522.644502	58.974288	48.572532
1519.188103	69.554095	48.577537
1515.633213	72.724026	48.582541
1512.224815	76.598809	48.587546
1508.363340	64.548437	48.592551
1504.849678	59.562260	48.597556
1502.112086	63.269359	48.602561
1498.206440	63.845867	48.607565
1494.387438	66.370385	48.612570
1490.557966	71.816628	48.617575
1487.452251	62.967353	48.622580
1484.087881	67.464859	48.627585
1480.733996	70.556052	48.632589
1477.182539	63.851544	48.637594
1473.354115	67.835995	48.642599
1470.195182	63.057196	48.647604
1466.808420	75.723700	48.652609
1463.086591	66.600170	48.657613
1459.576154	65.773761	48.662618
1456.292938	68.793845	48.667623
1452.701379	60.573844	48.672628
1449.088453	67.118988	48.677633
1445.694422	60.864538	48.682637
1442.116462	66.009049	48.687642
1438.628525	70.595393	48.692647
1435.211902	66.217369	48.697652
1432.043778	68.017335	48.702657
1428.137485	69.932197	48.707661
1424.998349	62.375759	48.712666
1420.745853	65.932683	48.717671
1417.715437	58.966756	48.722676
1414.171328	65.222785	48.727681
1410.679537	67.652088	48.732685
1407.255943	65.173372	48.737690
1403.760140	64.626260	48.742695
1400.254332	63.030359	48.747700
1396.780097	66.251018	48.752705
1393.145081	61.454585	48.757709
1389.874281	60.325134	48.762714
1386.396867	67.659095	48.767719
1382.663620	59.201738	48.772724
1378.764384	64.418404	48.777729
1375.508430	59.113729	48.782733
1372.412680	64.028166	48.787738
1368.287690	64.891925	48.792743
1365.317283	56.530967	48.797748
1361.864430	60.067834	48.802753
1358.452781	68.150846	48.807757
1355.110478	62.078180	48.812762
1351.178154	60.634092	48.817767
1347.735612	53.093259	48.822772
1344.066919	62.943656	48.827777
1340.239032	60.404493	48.832781
1337.432847	54.014272	48.837786
1333.775707	57.972071	48.842791
1330.665539	51.936045	48.847796
1326.773660	60.815126	48.852801
1323.056049	54.775574	48.857805
1319.732641	60.007017	48.862810
1316.254405	66.591313	48.867815
1312.655412	65.149128	48.872820
1309.274375	59.848113	48.877825
1305.831460	58.340508	48.882829
1302.591597	64.618787	48.887834
1298.327563	68.212319	48.892839
1295.188505	64.015734	48.897844
1291.874462	61.779404	48.902849
1288.216371	56.296894	48.907853
1284.666608	59.295204	48.912858
1280.869207	57.156257	48.917863
1277.833270	56.271830	48.922868
1274.482490	62.858434	48.927873
1270.254491	59.027498	48.932877
1267.221853	60.926609	48.937882
1263.582512	60.708733	48.942887
1260.465015	56.337959	48.947892
1256.795091	51.024973	48.952897
1253.225893	57.705683	48.957901
1249.984604	50.355001	48.962906
1246.012470	57.841897	48.967911
1242.587211	55.955072	48.972916
1239.093512	55.483580	48.977921
1235.726221	53.606716	48.982925
1232.573087	58.748386	48.987930
1228.872410	54.196313	48.992935
1225.551445	52.397659	48.997940
1221.557635	59.280502	49.002945
1217.815191	61.808946	49.007949
1214.777748	48.962846	49.012954
1211.216986	63.975407	49.017959
1207.848167	56.571814	49.022964
1203.913164	66.973023	49.027969
1200.655623	59.580583	49.032973
1197.391995	49.354428	49.037978
1193.869614	57.277511	49.042983
1190.532208	54.959411	49.047988
1186.729046	55.735133	49.052993
1183.052815	52.723143	49.057997
1179.527986	58.264350	49.063002
1175.957195	66.068425	49.068007
1172.773941	57.316694	49.073012
1169.187265	59.140703	49.078017
1165.793862	59.124997	49.083021
1162.128816	57.800679	49.088026
1158.405619	70.187356	49.093031
1155.154066	58.741303	49.098036
1151.554703	61.522722	49.103041
1148.159919	54.063073	49.108045
1144.745756	56.559406	49.113050
1140.978830	60.793732	49.118055
1137.787645	56.478736	49.123060
1134.397866	58.885855	49.128065
1130.557655	59.028285	49.133069
1127.399239	51.642576	49.138074
1123.574489	55.648627	49.143079
1120.170355	47.968982	49.148084
1116.699989	57.219047	49.153089
1113.254825	64.079773	49.158093
1109.951424	56.792561	49.163098
1106.291650	55.559177	49.168103
1102.602539	58.759522	49.173108
1098.962691	57.633766	49.178113
1095.203273	62.344644	49.183117
1092.134020	53.337908	49.188122
1088.581137	59.870559	49.193127
1085.360140	54.253608	49.198132
1081.867264	59.656973	49.203137
1077.819596	56.462374	49.208141
1074.396712	53.727333	49.213146
1070.756165	57.160562	49.218151
1067.833101	55.486647	49.223156
1063.959567	43.672377	49.228161
1060.358967	54.730197	49.233165
1057.269568	46.080940	49.238170
1054.026624	52.995606	49.243175
1050.266098	50.363745	49.248180
1046.637328	55.263092	49.253185
1042.761783	56.043770	49.258189
1039.475953	52.566080	49.263194
1035.933721	46.530917	49.268199
1032.636046	48.417518	49.273204
1029.512101	55.354790	49.278209
1025.537784	54.192524	49.283213
1022.373366	50.420697	49.288218
1018.527542	56.084644	49.293223
1015.096300	52.218313	49.298228
1011.439333	59.988351	49.303233
1007.597859	59.523565	49.308237
1004.540465	52.729579	49.313242
1000.886826	51.637620	49.318247
997.691406	56.728938	49.323252
994.074895	55.802038	49.328257
990.431196	56.768091	49.333261
987.401014	54.288301	49.338266
983.484838	61.393189	49.343271
980.031682	54.240041	49.348276
976.783492	57.289508	49.353281
973.058863	59.457706	49.358285
969.733677	48.548331	49.363290
966.013902	54.205316	49.368295
962.464076	49.965155	49.373300
958.914063	50.536986	49.378305
955.412277	55.675995	49.383309
952.185177	48.807199	49.388314
948.288988	50.065653	49.393319
945.038724	50.518062	49.398324
941.413268	51.680592	49.403329
938.064692	53.666872	49.408333
934.931267	54.015674	49.413338
931.099072	59.443395	49.418343
927.345713	52.200949	49.423348
923.444909	54.159300	49.428353
920.106242	51.148585	49.433357
917.186376	47.414634	49.438362
913.662685	52.968334	49.443367
910.089559	43.711048	49.448372
906.812251	50.763944	49.453377
902.835528	55.768085	49.458381
899.439096	51.719186	49.463386
895.939528	46.284833	49.468391
892.500545	55.583802	49.473396
889.009548	47.041381	49.478401
885.246378	52.363448	49.483405
881.788522	50.203341	49.488410
878.630740	54.456759	49.493415
874.889777	50.663971	49.498420
871.394626	46.728519	49.503425
868.191578	57.363800	49.508429
864.840166	49.343806	49.513434
860.902619	46.603491	49.518439
857.853051	41.950127	49.523444
854.012793	50.906609	49.528449
850.148369	47.145699	49.533453
846.710235	43.805638	49.538458
843.059232	49.597455	49.543463
839.965429	54.230049	49.548468
836.530776	56.770727	49.553473
832.924179	49.961025	49.558477
829.830151	44.150350	49.563482
825.540020	54.616339	49.568487
822.602301	54.419009	49.573492
818.700230	53.043050	49.578497
815.255015	57.179869	49.583501
811.954211	49.667687	49.588506
808.275472	58.330120	49.593511
804.794250	58.144631	49.598516
801.783908	46.534564	49.603521
797.872961	55.100268	49.608525
794.625573	52.483476	49.613530
790.765006	54.055937	49.618535
787.224907	56.768055	49.623540
784.123160	56.599426	49.628545
780.589091	59.117621	49.633549
777.040003	47.857173	49.638554
773.066714	53.689674	49.643559
769.771917	55.794146	49.648564
766.550431	51.389012	49.653569
762.796274	62.204998	49.658573
759.392591	51.959603	49.663578
755.897163	50.001509	49.668583
752.199904	52.953225	49.673588
748.413503	54.273706	49.678593
745.017471	64.103825	49.683597
741.982106	47.907166	49.688602
738.284733	56.768650	49.693607
735.178551	45.442429	49.698612
731.559482	48.261755	49.703617
727.615691	52.023788	49.708621
724.297403	52.211570	49.713626
720.944916	62.762555	49.718631
717.300008	51.877693	49.723636
713.836065	58.614814	49.728641
710.174159	52.269313	49.733645
707.377232	45.599344	49.738650
703.290421	50.405510	49.743655
699.889834	55.797698	49.748660
696.171908	51.330654	49.753665
692.310618	63.299080	49.758669
689.464362	52.008330	49.763674
685.905086	62.196048	49.768679
682.103316	56.710697	49.773684
678.909535	53.104837	49.778689
675.140445	57.447106	49.783693
671.811351	46.535240	49.788698
667.969041	55.068122	49.793703
664.553338	53.138758	49.798708
661.440620	48.995112	49.803713
657.860381	47.423549	49.808717
654.242331	44.535457	49.813722
650.363727	44.959166	49.818727
647.384248	52.035313	49.823732
643.841369	51.157108	49.828737
640.099860	53.318479	49.833741
636.981821	51.105505	49.838746
633.395089	49.190116	49.843751
630.236475	43.531894	49.848756
626.586019	38.010350	49.853761
622.414256	47.271544	49.858765
618.970049	38.908553	49.863770
615.018323	49.628747	49.868775
612.176771	41.462996	49.873780
608.779251	53.716718	49.878785
604.916008	54.881505	49.883789
601.850153	43.662928	49.888794
598.353036	55.315240	49.893799
595.049439	52.356058	49.898804
591.717510	45.484662	49.903809
587.589154	50.730732	49.908813
584.294540	39.630028	49.913818
580.651233	46.455187	49.918823
577.100319	47.659938	49.923828
573.195284	46.271825	49.928833
569.857672	49.344737	49.933837
566.733542	41.283095	49.938842
563.208506	54.920212	49.943847
559.726518	49.287031	49.948852
556.458214	43.721825	49.953857
552.431126	45.839080	49.958861
549.188462	42.164923	49.963866
545.775359	51.580095	49.968871
542.366013	45.853355	49.973876
538.646291	37.504798	49.978881
534.991477	48.355940	49.983885
531.782525	45.809131	49.988890
528.011053	47.987833	49.993895
524.704428	50.407375	49.998900
520.795096	45.900559	50.003905
517.294585	54.702935	50.008909
513.980392	42.928267	50.013914
510.715786	44.809772	50.018919
507.046953	42.132085	50.023924
503.613969	42.420004	50.028929
500.339773	48.333517	50.033933
496.345520	38.246561	50.038938
492.779182	45.774733	50.043943
489.620665	41.802755	50.048948
486.332310	46.598534	50.053953
482.837321	51.379028	50.058957
479.649643	41.735969	50.063962
475.742022	54.939115	50.068967
471.915631	52.083485	50.073972
468.181907	51.364726	50.078977
465.178667	55.919975	50.083981
461.447094	45.561182	50.088986
458.269946	50.387107	50.093991
454.327039	47.043433	50.098996
450.929132	46.310361	50.104001
447.118230	43.540909	50.109005
444.218648	38.396035	50.114010
440.433483	50.643670	50.119015
437.157818	46.095167	50.124020
433.601730	43.422085	50.129025
429.615669	51.249718	50.134029
426.677683	42.146749	50.139034
423.075972	53.258543	50.144039
419.684783	50.265569	50.149044
415.968091	48.844995	50.154049
412.588386	53.446202	50.159053
409.440156	42.851079	50.164058
405.675920	56.278671	50.169063
402.157137	50.214661	50.174068
398.571176	43.832091	50.179073
394.739054	54.989248	50.184077
391.407393	50.436815	50.189082
388.059356	50.369848	50.194087
384.302473	45.386921	50.199092
381.010609	46.722205	50.204097
377.081150	53.098399	50.209101
373.957876	46.820966	50.214106
370.329208	49.274841	50.219111
366.877054	44.057820	50.224116
363.414942	45.549321	50.229121
359.660875	51.566026	50.234125
356.471921	48.446669	50.239130
353.390469	48.379332	50.244135
349.428020	47.250122	50.249140
345.881979	45.907393	50.254145
342.052335	45.554753	50.259149
339.013796	38.776933	50.264154
335.270930	43.735230	50.269159
332.276375	54.939161	50.274164
328.713713	39.745334	50.279169
325.020581	48.571379	50.284173
321.953503	43.949295	50.289178
317.841433	47.829319	50.294183
314.356917	59.103205	50.299188
310.881428	43.418094	50.304193
307.417947	44.672541	50.309197
303.785038	44.947320	50.314202
300.468799	52.591591	50.319207
296.817371	53.201439	50.324212
293.712498	46.832573	50.329217
289.488458	55.801388	50.334221
286.150546	50.332483	50.339226
282.510654	46.878393	50.344231
279.218451	50.355542	50.349236
276.102380	55.766743	50.354241
272.380624	56.561545	50.359245
268.970225	52.480122	50.364250
265.378317	52.527067	50.369255
261.569881	53.063290	50.374260
258.510699	44.940975	50.379265
254.759794	53.140125	50.384269
251.562513	42.144561	50.389274
247.839665	48.630965	50.394279
244.289129	45.760902	50.399284
240.834022	47.219692	50.404289
237.504659	49.291637	50.409293
234.192318	46.431947	50.414298
230.285181	48.385044	50.419303
226.847789	44.763400	50.424308
223.608528	46.036731	50.429313
219.443374	53.227897	50.434317
216.183475	46.402304	50.439322
212.811826	56.772795	50.444327
209.281314	53.140340	50.449332
205.971245	46.904673	50.454337
202.213780	60.135074	50.459341
198.617519	48.562574	50.464346
195.392164	56.461616	50.469351
191.510726	48.508456	50.474356
188.095565	52.039559	50.479361
184.597555	56.023310	50.484365
181.523234	46.865685	50.489370
178.009393	49.459890	50.494375
174.447929	49.714073	50.499380
171.049362	50.502864	50.504385
167.157209	53.779212	50.509389
163.915602	50.981284	50.514394
160.103011	47.876796	50.519399
156.639318	46.284001	50.524404
153.103706	44.784659	50.529409
149.792486	50.912766	50.534413
146.194012	43.548296	50.539418
142.701801	58.043992	50.544423
138.934795	55.204484	50.549428
135.598915	51.658796	50.554433
132.136868	47.642385	50.559437
128.889201	51.897204	50.564442
124.948831	50.233100	50.569447
121.878864	41.115940	50.574452
118.191382	46.843899	50.579457
114.664412	53.068873	50.584461
111.502653	45.810417	50.589466
107.748937	45.933196	50.594471
104.349606	48.636128	50.599476
100.845323	46.480203	50.604481
97.002406	54.326708	50.609485
93.663758	41.220884	50.614490
90.237096	53.570903	50.619495
86.451577	45.134614	50.624500
83.369453	34.927896	50.629505
79.711730	45.055034	50.634509
75.923242	38.460461	50.639514
72.375080	46.526821	50.644519
69.220210	42.101940	50.649524
65.972412	43.563276	50.654529
62.240548	47.020318	50.659533
59.142822	35.734063	50.664538
55.198093	51.401162	50.669543
51.136061	44.510670	50.674548
48.369521	45.080855	50.679553
44.674945	36.013507	50.684557
41.398221	41.206135	50.689562
37.791210	46.121168	50.694567
33.860377	35.717581	50.699572
30.860317	40.088875	50.704577
26.915080	47.400839	50.709581
23.466971	41.256302	50.714586
19.818503	44.776292	50.719591
16.072539	43.012340	50.724596
13.046440	38.428220	50.729601
9.786896	41.438418	50.734605
6.307119	37.658904	50.739610
2.975090	42.110360	50.744615