Fri Aug 26 11:04:54 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
1.358975	98.364151	0.000000
1.355231	102.876319	0.005005
1.082514	96.515731	0.010010
1.177461	93.590581	0.015014
0.924480	84.844687	0.020019
0.743912	92.491098	0.025024
0.524843	78.092793	0.030029
-0.452769	78.390736	0.035034
-0.253246	64.616945	0.040038
-0.061043	62.695356	0.045043
-0.750656	53.612512	0.050048
-0.762222	52.760329	0.055053
-1.337008	48.560110	0.060058
-1.028368	38.005768	0.065062
-1.753776	39.207211	0.070067
-2.019110	30.093120	0.075072
-2.162047	23.794606	0.080077
-2.976731	14.259873	0.085082
-2.860151	10.727112	0.090086
-3.326166	14.308356	0.095091
-3.521784	16.474478	0.100096
-3.566141	14.963036	0.105101
-4.513585	11.991398	0.110106
-3.927325	11.286573	0.115110
-4.203592	1.965399	0.120115
-4.607499	11.250516	0.125120
-5.333838	-1.094628	0.130125
-5.664406	3.433600	0.135130
-5.385442	6.769142	0.140134
-5.480865	4.490559	0.145139
-6.218660	3.273740	0.150144
-6.829855	5.896857	0.155149
-7.141734	0.921750	0.160154
-7.089723	-3.603830	0.165158
-7.298582	-3.672345	0.170163
-7.537674	-0.300436	0.175168
-7.132577	-1.204836	0.180173
-7.222064	2.653128	0.185178
-7.874205	-1.576162	0.190182
-8.453440	-0.479735	0.195187
-8.451742	7.084478	0.200192
-8.435254	-1.640055	0.205197
-9.253509	9.098414	0.210202
-9.563630	-3.672188	0.215206
-9.647877	5.142391	0.220211
-10.010348	7.894455	0.225216
-9.828407	2.896243	0.230221
-10.421551	-0.760122	0.235226
-11.091408	-4.692433	0.240230
-11.385341	0.972166	0.245235
-11.662120	-10.519182	0.250240
-11.731883	5.771994	0.255245
-11.568826	4.668005	0.260250
-11.482059	-3.558122	0.265254
-11.612669	-0.627032	0.270259
-11.601817	-2.795615	0.275264
-11.812242	-1.652211	0.280269
-12.613596	0.820185	0.285274
-13.560085	-5.685389	0.290278
-14.217209	1.810563	0.295283
-13.872669	-4.699877	0.300288
-14.378240	-2.982190	0.305293
-14.567152	5.301374	0.310298
-14.254282	5.967847	0.315302
-14.368390	5.052540	0.320307
-14.315803	0.229487	0.325312
-14.193916	-4.927045	0.330317
-15.353302	-2.563414	0.335322
-15.803905	-1.449051	0.340326
-15.733382	0.729413	0.345331
-16.035023	5.961794	0.350336
-16.595895	-7.753656	0.355341
-17.121088	-1.932832	0.360346
-17.047004	-7.951923	0.365350
-16.854911	-2.397799	0.370355
-17.067628	-0.516909	0.375360
-17.167989	-2.769413	0.380365
-18.338914	-2.159808	0.385370
-18.479847	-0.865877	0.390374
-18.620710	0.073714	0.395379
-18.833697	-3.932895	0.400384
-18.917043	-4.843499	0.405389
-18.833643	5.874799	0.410394
-19.043870	-3.222544	0.415398
-19.903919	-3.983744	0.420403
-20.098652	-6.983992	0.425408
-19.958748	-5.094732	0.430413
-20.340310	-0.991985	0.435418
-20.023636	-0.022395	0.440422
-21.005132	-1.391087	0.445427
-21.583003	-4.872665	0.450432
-21.316643	-1.883164	0.455437
-21.699114	6.402064	0.460442
-21.682374	-0.256648	0.465446
-21.897063	-0.852584	0.470451
-22.417643	9.488372	0.475456
-22.925393	-1.324798	0.480461
-23.222271	1.692290	0.485466
-23.096870	8.788005	0.490470
-23.202650	0.661455	0.495475
-23.704271	12.748957	0.500480
-24.085523	6.171191	0.505485
-24.871120	7.673059	0.510490
-24.281210	0.399940	0.515494
-24.490124	4.121479	0.520499
-24.767521	3.335997	0.525504
-24.521303	1.586332	0.530509
-25.246978	-0.360011	0.535514
-25.672472	-9.116960	0.540518
-25.970029	-4.090855	0.545523
-25.857384	1.077021	0.550528
-26.270180	-6.495540	0.555533
-26.911293	5.506111	0.560538
-27.247557	-2.720587	0.565542
-27.195240	6.708620	0.570547
-27.625023	0.964124	0.575552
-27.598016	2.494489	0.580557
-27.876648	2.044546	0.585562
-27.965139	-5.287454	0.590566
-28.595589	9.619927	0.595571
-29.074046	9.916080	0.600576
-29.062384	-4.805970	0.605581
-29.225250	0.499711	0.610586
-29.074841	-0.842744	0.615590
-29.184657	0.607687	0.620595
-29.973658	-4.973313	0.625600
-30.390008	-4.990540	0.630605
-30.619268	3.640978	0.635610
-30.785072	0.035132	0.640614
-30.793259	-3.282052	0.645619
-30.952229	11.169120	0.650624
-31.358996	3.994236	0.655629
-31.925625	2.526149	0.660634
-31.883867	4.563564	0.665638
-31.894870	-1.268280	0.670643
-32.276674	-1.993215	0.675648
-32.697916	-2.503208	0.680653
-33.445368	6.158375	0.685658
-33.499704	4.683288	0.690662
-33.347457	8.231540	0.695667
-33.730941	8.300942	0.700672
-33.108811	6.840748	0.705677
-34.049951	1.843399	0.710682
-34.553727	6.936416	0.715686
-34.809673	9.361857	0.720691
-34.864272	7.127536	0.725696
-34.711619	-1.497978	0.730701
-35.452269	5.362432	0.735706
-35.920574	3.610127	0.740710
-36.182854	8.418779	0.745715
-36.205107	9.010884	0.750720
-36.175587	2.084435	0.755725
-36.593359	1.080373	0.760730
-36.943782	-0.655486	0.765734
-37.197778	10.308328	0.770739
-37.691213	4.380760	0.775744
-37.014813	-3.405680	0.780749
-37.869439	11.941553	0.785754
-38.439494	3.861981	0.790758
-38.668742	8.415562	0.795763
-39.149780	12.853329	0.800768
-38.982058	10.305992	0.805773
-39.319185	17.780598	0.810778
-39.010971	2.170840	0.815782
-39.526970	1.299127	0.820787
-40.215481	4.443628	0.825792
-40.457727	0.061938	0.830797
-41.013423	5.716675	0.835802
-40.732012	1.484397	0.840806
-40.998788	6.081784	0.845811
-40.849198	9.143249	0.850816
-40.679441	-0.263185	0.855821
-41.905726	5.258690	0.860826
-41.814896	6.026170	0.865830
-41.942819	-2.375330	0.870835
-42.391348	0.504024	0.875840
-42.550126	-2.128513	0.880845
-42.824472	0.252338	0.885850
-42.856827	0.045614	0.890854
-43.013177	4.132278	0.895859
-43.823741	-1.290346	0.900864
-44.281062	0.106628	0.905869
-44.863343	7.515000	0.910874
-44.877757	-12.710886	0.915878
-44.561659	-1.453043	0.920883
-44.554928	-3.098983	0.925888
-44.726844	-3.242850	0.930893
-45.332100	3.394005	0.935898
-45.810163	5.559811	0.940902
-46.094065	-6.803592	0.945907
-46.474930	-1.416515	0.950912
-46.150126	-8.221261	0.955917
-46.638086	-0.403650	0.960922
-47.311785	-2.611176	0.965926
-47.474305	-0.323664	0.970931
-47.733912	8.600471	0.975936
-47.777207	-0.801263	0.980941
-47.821198	-0.879629	0.985946
-47.723348	4.274732	0.990950
-48.508760	4.526932	0.995955
-49.092929	1.805610	1.000960
-49.038041	-2.922889	1.005965
-49.284142	5.999142	1.010970
-49.061450	1.301460	1.015974
-49.422280	-8.082466	1.020979
-50.308948	6.731931	1.025984
-50.456516	0.769496	1.030989
-50.702808	7.932572	1.035994
-50.984560	0.073861	1.040998
-50.428273	4.163459	1.046003
-51.068212	4.544864	1.051008
-51.436835	-1.674208	1.056013
-52.184819	6.911530	1.061018
-52.248387	0.765179	1.066022
-52.104702	-8.384099	1.071027
-52.302200	-2.358044	1.076032
-52.430991	-4.723175	1.081037
-52.941598	8.770377	1.086042
-53.592469	9.387595	1.091046
-53.930616	1.806573	1.096051
-54.046153	6.370921	1.101056
-54.228377	-0.788303	1.106061
-54.260797	0.855715	1.111066
-53.884752	-0.436454	1.116070
-54.007960	-0.891615	1.121075
-55.070674	9.856442	1.126080
-55.113759	-1.247365	1.131085
-55.298952	10.607373	1.136090
-55.541223	3.527097	1.141094
-56.104344	-1.168451	1.146099
-56.638466	6.865151	1.151104
-56.467681	-0.766637	1.156109
-56.752701	7.569853	1.161114
-56.620268	-2.871606	1.166118
-56.898629	-7.421671	1.171123
-57.741714	0.236105	1.176128
-57.869732	-3.239586	1.181133
-58.474607	-1.566546	1.186138
-58.342248	-8.648201	1.191142
-58.352467	-8.542008	1.196147
-58.533956	-4.517868	1.201152
-58.884048	-2.334025	1.206157
-59.381918	5.649641	1.211162
-59.693481	-5.355415	1.216166
-59.769816	-3.321760	1.221171
-59.906977	-3.081910	1.226176
-60.040986	-3.785316	1.231181
-60.946459	0.300931	1.236186
-61.278191	-0.580490	1.241190
-61.125165	4.150842	1.246195
-61.438283	1.618263	1.251200
-61.453752	0.222544	1.256205
-61.653391	-0.594026	1.261210
-61.607166	-5.362303	1.266214
-61.850449	-9.974774	1.271219
-62.755865	7.518982	1.276224
-62.628090	-2.402914	1.281229
-62.952308	6.126334	1.286234
-63.148267	-8.047709	1.291238
-63.227617	-5.339729	1.296243
-64.068596	-7.195353	1.301248
-63.889113	-7.162987	1.306253
-64.024252	4.041734	1.311258
-64.384724	-1.928678	1.316262
-64.791393	0.703721	1.321267
-65.513258	0.658136	1.326272
-65.560466	-3.478683	1.331277
-65.715089	3.404372	1.336282
-65.900665	1.260045	1.341286
-65.348242	-7.582727	1.346291
-66.031923	-1.696101	1.351296
-66.200027	0.003843	1.356301
-66.800266	1.457869	1.361306
-66.472368	-1.528843	1.366310
-67.058945	0.033784	1.371315
-67.808927	1.805344	1.376320
-68.225911	0.437341	1.381325
-68.761926	6.323123	1.386330
-68.671125	4.980457	1.391334
-68.865625	-2.885509	1.396339
-68.569808	-4.721987	1.401344
-68.745335	-2.100268	1.406349
-68.741158	5.216790	1.411354
-68.888299	-5.000809	1.416358
-69.527434	-2.458761	1.421363
-70.127120	-1.662859	1.426368
-70.291688	-3.383363	1.431373
-71.006467	4.086764	1.436378
-70.934906	-2.710190	1.441382
-71.221561	-3.060810	1.446387
-71.550110	7.085732	1.451392
-71.257970	-0.049276	1.456397
-71.466418	2.413059	1.461402
-71.610373	0.186326	1.466406
-72.585442	1.493077	1.471411
-73.109255	7.003650	1.476416
-73.191271	2.622321	1.481421
-73.376352	4.859564	1.486426
-73.731792	-0.637085	1.491430
-73.514016	-1.990029	1.496435
-73.452135	5.643900	1.501440
-73.135157	4.544418	1.506445
-73.799518	15.562636	1.511450
-74.809398	9.794571	1.516454
-74.591682	1.918202	1.521459
-74.783008	5.931221	1.526464
-75.249556	3.213732	1.531469
-75.894920	5.399259	1.536474
-76.418006	11.400084	1.541478
-76.515216	3.338640	1.546483
-76.584082	4.804841	1.551488
-76.106882	0.412370	1.556493
-76.487907	1.522228	1.561498
-76.650819	-7.142729	1.566502
-76.932817	0.782013	1.571507
-77.454036	0.056641	1.576512
-77.564178	2.000651	1.581517
-78.049169	1.038692	1.586522
-78.501951	-6.692148	1.591526
-78.578701	-1.026567	1.596531
-78.791134	0.420859	1.601536
-78.805833	4.561395	1.606541
-78.864889	6.981489	1.611546
-79.972174	4.072708	1.616550
-80.273986	10.918574	1.621555
-80.946445	4.753137	1.626560
-80.685977	-3.996724	1.631565
-80.570081	6.175526	1.636570
-80.833972	-1.100689	1.641574
-80.855207	2.610609	1.646579
-80.984365	3.162413	1.651584
-81.221985	-4.155855	1.656589
-81.724497	0.800925	1.661594
-81.517926	0.411473	1.666598
-82.030101	1.551242	1.671603
-82.643824	7.357378	1.676608
-83.265651	1.731369	1.681613
-83.272957	5.870754	1.686618
-83.654672	1.317798	1.691622
-83.429314	-3.218951	1.696627
-83.399301	10.070206	1.701632
-83.404153	9.087271	1.706637
-84.590640	6.488205	1.711642
-84.903951	5.920280	1.716646
-84.835547	2.426660	1.721651
-85.376556	-0.462725	1.726656
-85.410880	-3.785330	1.731661
-85.225027	-3.889992	1.736666
-85.204711	-1.207021	1.741670
-86.031731	0.497443	1.746675
-86.500220	5.360345	1.751680
-86.457559	-0.005306	1.756685
-86.753641	3.116058	1.761690
-87.122031	-1.929336	1.766694
-87.588169	-3.691467	1.771699
-88.331205	7.063757	1.776704
-88.300282	5.031249	1.781709
-88.295821	5.780540	1.786714
-88.332055	-5.507818	1.791718
-88.203535	1.264712	1.796723
-88.422681	5.873664	1.801728
-88.445734	-4.347437	1.806733
-89.334925	2.586717	1.811738
-89.711958	3.265698	1.816742
-89.809260	-5.241801	1.821747
-90.033543	0.861188	1.826752
-90.339480	1.633499	1.831757
-90.255900	8.283320	1.836762
-90.576222	7.612087	1.841766
-90.638159	-1.552631	1.846771
-91.499532	-0.307873	1.851776
-91.903512	1.131414	1.856781
-92.106664	2.476159	1.861786
-92.511956	5.041908	1.866790
-92.370421	-1.794413	1.871795
-92.665027	1.608285	1.876800
-92.459076	8.650326	1.881805
-92.353432	0.955918	1.886810
-93.485493	-0.243800	1.891814
-93.860877	-0.276895	1.896819
-93.974899	-4.694365	1.901824
-94.117401	-4.864957	1.906829
-94.174060	6.485725	1.911834
-94.772613	9.885130	1.916838
-94.883956	2.895200	1.921843
-95.666190	5.965713	1.926848
-95.957576	0.794438	1.931853
-95.888835	7.120713	1.936858
-95.670583	7.979081	1.941862
-96.047776	1.289963	1.946867
-96.241920	12.054635	1.951872
-95.705339	3.866036	1.956877
-96.373809	5.261087	1.961882
-96.558363	-0.369731	1.966886
-96.983463	-7.880261	1.971891
-98.067874	6.240447	1.976896
-98.263290	-0.802828	1.981901
-98.554145	7.971150	1.986906
-98.906538	4.403850	1.991910
-98.338045	1.800441	1.996915
-98.386589	-1.352840	2.006912
-98.701160	-3.147053	2.016909
-98.658347	-2.266361	2.026906
-97.588852	-5.185204	2.036902
-97.074077	4.792473	2.046899
-96.387521	2.044123	2.056896
-95.990482	5.704747	2.066893
-95.839095	0.553085	2.076890
-94.980380	2.570649	2.086886
-94.738607	2.663284	2.096883
-94.258918	2.801235	2.106880
-93.446585	3.406895	2.116877
-93.038599	4.709051	2.126874
-92.780479	4.083242	2.136870
-91.896412	7.129528	2.146867
-91.590948	5.150078	2.156864
-91.417310	3.349538	2.166861
-90.846140	-0.948854	2.176858
-90.195217	-4.692646	2.186854
-89.408894	3.769774	2.196851
-89.298566	1.789030	2.206848
-88.510554	2.160900	2.216845
-87.835776	-1.859029	2.226842
-87.862796	-1.629511	2.236838
-87.370182	3.802811	2.246835
-86.517294	1.456201	2.256832
-86.265816	2.329746	2.266829
-85.086836	7.154705	2.276826
-84.885449	1.577121	2.286822
-84.764835	-0.585783	2.296819
-84.474403	0.915235	2.306816
-83.791153	1.436460	2.316813
-82.633969	1.820538	2.326810
-82.318556	-0.502572	2.336806
-82.237431	3.362458	2.346803
-81.780621	3.833412	2.356800
-80.932788	3.492740	2.366797
-80.555989	4.565342	2.376794
-80.449429	-5.530444	2.386790
-79.696487	-6.828823	2.396787
-78.874281	8.055261	2.406784
-78.390048	4.546489	2.416781
-77.684936	1.725561	2.426778
-77.551728	4.423106	2.436774
-77.681134	0.645594	2.446771
-76.610598	2.744215	2.456768
-76.142501	12.206497	2.466765
-75.188221	2.650266	2.476762
-74.866567	1.171958	2.486758
-74.825932	7.061114	2.496755
-73.981491	0.046639	2.506752
-73.559230	4.637807	2.516749
-73.464924	1.889808	2.526746
-72.087993	-5.584530	2.536742
-71.908405	0.919695	2.546739
-71.895465	4.909379	2.556736
-71.035812	9.768221	2.566733
-70.527992	0.968895	2.576730
-70.053659	-2.440136	2.586726
-69.282332	-6.094973	2.596723
-69.047859	0.296173	2.606720
-68.825292	0.670556	2.616717
-67.956245	7.368365	2.626714
-67.364497	5.182788	2.636710
-67.277897	4.333437	2.646707
-66.284958	-1.342051	2.656704
-66.285514	-7.052910	2.666701
-65.863973	-4.637837	2.676698
-64.802983	-2.629592	2.686694
-64.665433	-2.590418	2.696691
-63.509698	-1.439531	2.706688
-63.518721	-3.091258	2.716685
-63.206147	1.396615	2.726682
-62.490731	-11.622719	2.736678
-61.596125	-13.497500	2.746675
-61.598203	-8.441136	2.756672
-61.411030	-0.778717	2.766669
-60.435930	-7.195833	2.776666
-60.232685	-5.066708	2.786662
-59.366106	-8.375258	2.796659
-58.922043	-6.125244	2.806656
-58.984517	-2.592637	2.816653
-57.734780	-7.617549	2.826650
-57.379454	-6.212163	2.836646
-57.215706	-8.128367	2.846643
-56.262927	-5.054767	2.856640
-55.840111	-0.210271	2.866637
-55.317351	-5.121993	2.876634
-55.335381	-0.563638	2.886630
-54.602055	-3.423803	2.896627
-54.172446	-5.932580	2.906624
-53.019381	2.399884	2.916621
-52.702447	1.207404	2.926618
-52.397378	-2.007385	2.936614
-52.414067	1.584615	2.946611
-51.763281	5.668216	2.956608
-51.078535	3.642383	2.966605
-50.069254	2.573346	2.976602
-50.000974	-0.677432	2.986598
-49.681401	1.230849	2.996595
-49.290393	-1.313099	3.006592
-48.766376	3.959120	3.016589
-47.474591	5.959941	3.026586
-47.513176	7.632561	3.036582
-47.060116	1.173183	3.046579
-46.770312	1.895047	3.056576
-45.849369	2.214544	3.066573
-45.346089	9.707379	3.076570
-45.194479	9.981941	3.086566
-44.563624	3.757798	3.096563
-44.243454	10.499891	3.106560
-43.033705	6.235114	3.116557
-42.863184	6.246980	3.126554
-42.885318	7.850517	3.136550
-41.761217	6.000188	3.146547
-41.747494	10.144969	3.156544
-41.044945	0.266815	3.166541
-40.332646	3.301835	3.176538
-40.288900	7.061818	3.186534
-39.185659	8.116346	3.196531
-38.911072	9.680019	3.206528
-38.418242	5.916492	3.216525
-38.291719	4.867696	3.226522
-37.276432	3.294061	3.236518
-36.950884	3.595391	3.246515
-35.960686	7.360062	3.256512
-35.741518	9.673604	3.266509
-35.599863	11.416360	3.276506
-35.397323	6.636852	3.286502
-34.278203	7.324623	3.296499
-33.995526	9.675793	3.306496
-33.438918	8.655064	3.316493
-32.702269	4.467116	3.326490
-32.563775	2.447141	3.336486
-32.356023	5.709601	3.346483
-31.225922	3.570078	3.356480
-30.941548	3.180927	3.366477
-30.277806	8.969901	3.376474
-29.788571	3.854328	3.386470
-29.720021	1.794561	3.396467
-28.737237	8.012182	3.406464
-28.197303	6.027901	3.416461
-28.134176	9.664495	3.426458
-27.712164	10.444967	3.436454
-26.796890	-0.251898	3.446451
-26.290740	-0.761107	3.456448
-26.350864	7.063363	3.466445
-25.532308	0.943039	3.476442
-24.857139	2.802291	3.486438
-23.861682	-2.540980	3.496435
-23.566181	5.959856	3.506432
-23.400852	4.369677	3.516429
-23.329306	1.688575	3.526426
-22.380384	2.076573	3.536422
-22.185444	0.076319	3.546419
-21.223439	4.573949	3.556416
-20.768988	2.321054	3.566413
-20.342668	-0.117523	3.576410
-20.338360	2.470218	3.586406
-19.836589	4.527523	3.596403
-18.644664	9.169915	3.606400
-17.973724	6.870641	3.616397
-17.939490	-1.458988	3.626394
-17.736792	-5.443426	3.636390
-16.804852	-0.012981	3.646387
-16.439987	3.069800	3.656384
-15.980349	9.783844	3.666381
-15.153354	5.331581	3.676378
-14.765698	3.190452	3.686374
-14.506806	-7.787502	3.696371
-14.189784	5.347487	3.706368
-13.585811	8.443724	3.716365
-12.787599	10.708291	3.726362
-11.765433	5.946883	3.736358
-11.615059	10.247780	3.746355
-11.588539	8.976976	3.756352
-11.379879	9.179302	3.766349
-10.432634	11.322467	3.776346
-9.986010	1.591859	3.786342
-9.105657	11.103996	3.796339
-8.878060	7.996298	3.806336
-8.746266	10.396303	3.816333
-7.990793	2.445368	3.826330
-7.440723	11.213839	3.836326
-6.487969	11.604409	3.846323
-6.234936	13.225290	3.856320
-6.098913	19.834508	3.866317
-5.717553	21.736341	3.876314
-5.229079	25.347893	3.886310
-4.392272	31.414030	3.896307
-4.086434	33.467001	3.906304
-3.404139	42.686888	3.916301
-2.939849	48.959914	3.926298
-2.578557	51.083446	3.936294
-2.034294	61.623593	3.946291
-1.866309	65.490954	3.956288
-1.349649	77.147274	3.966285
-1.030716	92.515267	3.976282
-0.639682	104.710669	3.986278
0.000000	106.117972	3.991283
0.204987	123.862892	3.996288
0.418460	134.067485	4.001293
0.668192	133.497309	4.006298
0.943807	134.969996	4.011302
0.766264	131.422896	4.016307
1.038912	136.474154	4.021312
0.786963	138.528841	4.026317
0.889892	134.647015	4.031322
0.577636	138.764313	4.036326
0.948713	137.327379	4.041331
0.993282	140.186927	4.046336
0.658523	142.146943	4.051341
0.888297	135.401228	4.056346
0.580911	146.715117	4.061350
1.059415	143.091180	4.066355
1.774646	151.806664	4.071360
1.299595	150.504633	4.076365
1.219934	139.849342	4.081370
1.173333	133.390261	4.086374
1.335230	133.770206	4.091379
1.208667	140.598330	4.096384
0.902744	134.192279	4.101389
1.443597	128.283959	4.106394
1.019884	139.859558	4.111398
1.694670	135.566000	4.116403
1.249055	143.351773	4.121408
1.112062	145.958024	4.126413
1.427818	142.827649	4.131418
1.055260	145.565486	4.136422
1.385284	137.481747	4.141427
1.026114	137.667582	4.146432
1.061571	144.815321	4.151437
1.207119	139.088765	4.156442
1.023973	145.675771	4.161446
1.379802	138.505478	4.166451
1.252437	139.218354	4.171456
0.974579	135.639418	4.176461
1.137439	137.306826	4.181466
1.113636	137.775794	4.186470
0.985013	136.290116	4.191475
1.281713	137.829121	4.196480
0.946015	137.163438	4.201485
1.538634	144.562941	4.206490
1.646066	150.753538	4.211494
1.369619	144.994610	4.216499
1.477917	140.877835	4.221504
1.314650	130.643680	4.226509
1.418547	140.261077	4.231514
1.288665	141.720971	4.236518
1.427238	148.659673	4.241523
2.009167	152.144219	4.246528
1.775535	155.081884	4.251533
2.045290	142.768206	4.256538
1.530590	143.155422	4.261542
1.615510	139.276399	4.266547
1.602363	147.374480	4.271552
1.387164	146.247121	4.276557
1.470366	141.514173	4.281562
1.337785	145.157420	4.286566
1.142391	145.795470	4.291571
1.135743	141.968666	4.296576
1.071589	152.608791	4.301581
1.388157	160.503686	4.306586
1.943551	165.390710	4.311590
1.975052	162.658921	4.316595
2.162264	152.926990	4.321600
1.468187	145.474085	4.326605
1.514284	134.773907	4.331610
1.754046	148.571507	4.336614
1.564421	156.750852	4.341619
1.998963	152.301712	4.346624
1.837428	148.679352	4.351629
1.794340	141.840080	4.356634
1.276951	142.892085	4.361638
1.514799	144.652220	4.366643
2.011142	154.233831	4.371648
1.760394	151.957266	4.376653
2.047858	158.034417	4.381658
1.774759	150.079377	4.386662
1.786611	155.987473	4.391667
1.889216	154.684086	4.396672
2.027908	159.455658	4.401677
2.017433	151.276235	4.406682
1.750782	143.073428	4.411686
1.734069	144.797269	4.416691
1.767671	150.939253	4.421696
2.256716	149.607334	4.426701
2.012074	150.338471	4.431706
1.531821	145.076335	4.436710
1.720709	154.288211	4.441715
2.304313	160.857079	4.446720
2.030845	169.074793	4.451725
2.070549	172.874715	4.456730
2.157967	161.854883	4.461734
1.932433	156.312645	4.466739
2.121330	157.789345	4.471744
1.706594	162.128243	4.476749
2.081414	159.855516	4.481754
2.228697	169.956543	4.486758
2.017319	157.755730	4.491763
2.301843	167.354510	4.496768
2.207840	159.441182	4.501773
1.954479	143.523273	4.506778
1.821226	153.655315	4.511782
2.177255	159.164984	4.516787
1.881015	160.831111	4.521792
1.576489	162.349836	4.526797
1.927053	166.569579	4.531802
1.513934	159.528493	4.536806
1.505080	166.543938	4.541811
2.333092	173.517671	4.546816
2.641877	182.188887	4.551821
2.399000	166.740713	4.556826
2.113783	169.300444	4.561830
2.298130	168.515826	4.566835
2.274772	158.446528	4.571840
1.823113	164.812763	4.576845
2.472538	169.441544	4.581850
2.577338	177.682623	4.586854
2.339974	175.005348	4.591859
2.148176	169.951387	4.596864
2.301208	177.343418	4.601869
2.498511	169.084181	4.606874
2.662523	166.306450	4.611878
2.320865	172.196828	4.616883
2.454108	168.787989	4.621888
1.803247	173.517985	4.626893
2.347971	174.021819	4.631898
2.730241	182.362063	4.636902
2.694216	180.048900	4.641907
2.893613	175.747093	4.646912
2.386876	175.642700	4.651917
2.443124	169.936366	4.656922
2.608942	173.409775	4.661926
1.990237	168.279918	4.666931
2.491550	176.285257	4.671936
2.331015	185.238350	4.676941
2.765119	179.523800	4.681946
2.922618	180.341018	4.686950
2.578724	180.198616	4.691955
2.346501	168.953308	4.696960
2.396462	186.542098	4.701965
2.668620	182.285908	4.706970
2.492023	183.487330	4.711974
2.927162	185.137660	4.716979
3.018959	188.299902	4.721984
2.215412	186.254932	4.726989
2.723338	190.254032	4.731994
2.628392	191.515507	4.736998
2.580236	191.380841	4.742003
2.956886	182.878544	4.747008
3.064178	185.921317	4.752013
2.490638	177.927624	4.757018
2.665718	187.530800	4.762022
3.020119	186.223006	4.767027
3.091225	187.461790	4.772032
2.551549	174.340832	4.777037
2.527337	172.838895	4.782042
2.616868	179.032290	4.787046
2.509976	182.747473	4.792051
2.926728	183.223777	4.797056
2.533721	195.338784	4.802061
2.785565	187.333632	4.807066
2.827773	190.199882	4.812070
2.385899	182.780458	4.817075
2.894584	188.263205	4.822080
2.791814	191.667708	4.827085
3.379689	177.263903	4.832090
2.821112	181.147486	4.837094
2.850681	184.208688	4.842099
3.134525	181.450261	4.847104
2.993051	179.722978	4.852109
3.076984	181.032529	4.857114
2.878205	186.081273	4.862118
2.897757	178.947503	4.867123
2.993213	175.433817	4.872128
3.103119	192.329926	4.877133
3.270365	184.157618	4.882138
3.309530	185.176754	4.887142
2.881173	180.950540	4.892147
3.150628	176.100001	4.897152
2.858236	191.505381	4.902157
3.049199	172.129967	4.907162
2.853039	180.731109	4.912166
3.063264	180.929528	4.917171
3.261696	181.775174	4.922176
2.955845	179.080089	4.927181
3.226189	183.169961	4.932186
3.064312	182.372812	4.937190
3.279980	181.975612	4.942195
3.332959	186.453660	4.947200
3.069307	192.186370	4.952205
3.309725	182.594832	4.957210
3.106456	189.548810	4.962214
3.447051	202.561979	4.967219
3.449067	188.910591	4.972224
3.157566	186.883970	4.977229
3.157972	183.527447	4.982234
3.349703	190.486362	4.987238
3.368244	197.380498	4.992243
3.607309	199.070848	4.997248
2.912021	199.176141	5.002253
2.795468	202.487882	5.007258
3.483943	211.561894	5.012262
3.563619	212.596870	5.017267
3.550658	206.388783	5.022272
3.165004	209.369108	5.027277
3.618306	210.924865	5.032282
3.638164	207.467235	5.037286
3.491811	209.923096	5.042291
3.768795	204.808791	5.047296
3.497421	209.476548	5.052301
3.487945	205.732427	5.057306
3.240815	205.005496	5.062310
3.620658	212.627977	5.067315
3.721094	203.444192	5.072320
3.566568	210.453863	5.077325
3.715354	197.826794	5.082330
2.989096	201.559324	5.087334
3.475910	206.194451	5.092339
3.694993	208.188463	5.097344
3.475176	213.291109	5.102349
3.584660	202.948008	5.107354
4.140269	214.491397	5.112358
3.852385	209.730789	5.117363
3.892831	194.896523	5.122368
3.498015	202.908525	5.127373
3.577741	190.336506	5.132378
3.557597	195.493478	5.137382
3.652170	203.394483	5.142387
3.912320	203.433273	5.147392
3.535200	209.069762	5.152397
3.956340	202.917471	5.157402
3.670928	207.793053	5.162406
3.451188	210.168593	5.167411
4.020372	196.492166	5.172416
3.784916	209.718413	5.177421
3.580950	202.198665	5.182426
3.731991	204.785388	5.187430
3.430003	208.296840	5.192435
3.752005	201.258336	5.197440
3.693784	203.460034	5.202445
3.767902	208.320765	5.207450
3.802768	206.790645	5.212454
3.591173	207.241398	5.217459
3.937690	204.982563	5.222464
3.620806	204.842282	5.227469
3.649796	200.699877	5.232474
3.930787	209.223578	5.237478
3.641597	206.646114	5.242483
4.093173	212.087141	5.247488
3.916137	222.096328	5.252493
4.230416	221.715411	5.257498
3.942986	207.258044	5.262502
3.847743	214.900713	5.267507
4.228882	218.862614	5.272512
4.039607	224.836849	5.277517
4.357875	219.478836	5.282522
3.964188	209.796191	5.287526
3.878877	207.006654	5.292531
4.200204	210.322984	5.297536
3.733603	207.975619	5.302541
4.272448	225.393419	5.307546
4.356533	229.186443	5.312550
4.120355	218.131540	5.317555
4.444966	210.377634	5.322560
4.051617	211.593824	5.327565
4.157911	201.627699	5.332570
4.141607	208.751886	5.337574
4.210460	222.427460	5.342579
4.432650	216.065701	5.347584
3.964964	209.453860	5.352589
4.023739	221.634582	5.357594
4.290674	219.467227	5.362598
4.513699	220.011660	5.367603
4.443100	216.738950	5.372608
4.141824	220.111092	5.377613
4.411226	221.799884	5.382618
4.350667	214.099619	5.387622
4.086440	210.904514	5.392627
4.444734	213.822793	5.397632
4.028373	220.544211	5.402637
4.138468	213.908846	5.407642
4.395730	210.721130	5.412646
4.343291	223.441176	5.417651
4.427287	222.482359	5.422656
4.114915	230.465718	5.427661
4.324362	219.575545	5.432666
4.414291	215.755834	5.437670
4.373886	227.774836	5.442675
4.350450	222.792720	5.447680
4.213027	230.755168	5.452685
4.302557	224.945560	5.457690
4.223642	230.804540	5.462694
4.258495	224.797805	5.467699
4.571503	216.454093	5.472704
4.332221	228.542024	5.477709
4.498028	240.829478	5.482714
5.005823	239.099173	5.487718
4.493687	234.987229	5.492723
4.278164	220.996372	5.497728
4.312557	232.418449	5.502733
4.889593	237.985480	5.507738
4.976864	240.768794	5.512742
4.994205	244.489957	5.517747
4.833571	234.343915	5.522752
4.387788	235.805547	5.527757
4.551752	224.767431	5.532762
4.529319	234.287492	5.537766
4.548013	235.730588	5.542771
4.809518	247.639323	5.547776
4.919374	237.840299	5.552781
4.784127	237.804612	5.557786
4.793089	229.555689	5.562790
4.272275	233.155000	5.567795
5.105709	239.811546	5.572800
5.039289	241.688666	5.577805
4.744514	231.626785	5.582810
4.603455	230.139872	5.587814
5.073540	244.872938	5.592819
4.917638	234.909653	5.597824
4.571749	236.178565	5.602829
4.634931	235.900017	5.607834
5.076238	242.801111	5.612838
5.071234	250.907463	5.617843
4.952327	242.846118	5.622848
4.762820	244.353269	5.627853
4.820123	244.901359	5.632858
5.046945	241.924015	5.637862
5.056374	247.962231	5.642867
4.991818	236.678119	5.647872
4.971257	246.311788	5.652877
4.846666	245.761925	5.657882
4.850701	248.437979	5.662886
5.005527	248.600733	5.667891
4.923093	244.988183	5.672896
4.868484	246.398402	5.677901
4.961762	242.954644	5.682906
5.010452	247.006277	5.687910
4.536141	254.072082	5.692915
4.987889	248.237706	5.697920
5.032820	245.443703	5.702925
5.126906	245.315364	5.707930
5.195735	247.250518	5.712934
4.708679	247.218989	5.717939
5.055470	250.632599	5.722944
5.238539	246.621214	5.727949
5.125516	243.943551	5.732954
4.882072	239.486057	5.737958
5.119570	258.247921	5.742963
5.768366	265.227448	5.747968
5.186187	258.845382	5.752973
5.123562	254.419842	5.757978
5.098825	255.040815	5.762982
5.053109	261.388171	5.767987
5.391157	265.995858	5.772992
5.350060	272.968910	5.777997
5.592598	273.076880	5.783002
5.670723	255.133114	5.788006
5.347178	251.801708	5.793011
5.312533	248.226008	5.798016
5.122142	251.928897	5.803021
5.219672	249.629730	5.808026
5.583088	266.103633	5.813030
5.370238	258.341640	5.818035
5.398332	243.771843	5.823040
5.142367	252.992923	5.828045
5.296787	262.115312	5.833050
5.616201	264.115854	5.838054
5.413475	263.546519	5.843059
5.619712	274.084507	5.848064
5.620345	277.561510	5.853069
5.247274	268.233122	5.858074
5.592643	266.132642	5.863078
5.189411	270.817781	5.868083
6.122685	260.672245	5.873088
5.415231	268.799391	5.878093
5.466951	275.153728	5.883098
5.867870	275.793848	5.888102
5.496461	266.354472	5.893107
5.626065	264.866542	5.898112
5.731954	267.931694	5.903117
5.659237	263.321064	5.908122
5.831211	249.342617	5.913126
5.629071	250.386672	5.918131
5.715729	246.035965	5.923136
5.537944	248.537853	5.928141
5.569318	262.567299	5.933146
5.593612	256.669763	5.938150
5.823529	275.160748	5.943155
5.947218	265.565194	5.948160
5.678553	261.380536	5.953165
5.614328	260.795964	5.958170
6.010501	268.355816	5.963174
5.613012	265.197268	5.968179
5.705710	265.486752	5.973184
5.738362	267.528779	5.978189
5.771225	274.721266	5.983194
5.565340	284.972257	5.988198
5.414895	285.103449	5.993203
5.340463	272.346571	5.998208
5.510897	280.099760	6.003213
5.628964	277.889140	6.008218
5.817207	283.896362	6.013222
6.006499	286.948532	6.018227
5.852857	285.327534	6.023232
5.591570	280.537456	6.028237
5.866159	280.216500	6.033242
5.867320	277.707712	6.038246
5.687823	283.632989	6.043251
5.822708	267.939251	6.048256
5.893491	272.183600	6.053261
5.974868	275.822034	6.058266
6.083898	276.463309	6.063270
5.894382	277.986282	6.068275
6.003387	281.680526	6.073280
6.072286	280.474125	6.078285
6.080382	279.530285	6.083290
6.035757	268.689131	6.088294
5.733813	274.035531	6.093299
5.824091	277.235990	6.098304
5.934869	276.310965	6.103309
5.937717	280.075520	6.108314
6.106965	288.271814	6.113318
6.016518	283.319097	6.118323
6.444523	273.309170	6.123328
5.716120	267.592097	6.128333
5.501831	259.918911	6.133338
5.664782	254.338302	6.138342
5.683961	265.958919	6.143347
5.951746	270.457326	6.148352
5.838542	280.361697	6.153357
5.939301	279.966568	6.158362
5.861323	271.943129	6.163366
5.877562	267.147809	6.168371
5.951688	259.562593	6.173376
5.764236	264.460902	6.178381
5.545465	260.822121	6.183386
6.141354	266.636156	6.188390
5.442788	271.781722	6.193395
5.838862	271.606364	6.198400
5.508396	281.471797	6.203405
5.527518	279.915649	6.208410
6.015596	277.960624	6.213414
5.454715	277.434398	6.218419
5.902742	285.476556	6.223424
5.556447	286.910047	6.228429
5.607293	279.575215	6.233434
5.879381	285.544075	6.238438
5.663145	287.982353	6.243443
5.812236	280.322182	6.248448
5.919292	290.271357	6.253453
5.691169	293.973802	6.258458
6.014864	283.341043	6.263462
5.597231	294.744956	6.268467
5.842759	287.800581	6.273472
6.054920	283.705565	6.278477
5.873748	292.551196	6.283482
6.064491	293.559393	6.288486
5.988058	290.164195	6.293491
6.166777	288.636979	6.298496
6.126188	284.087779	6.303501
5.958815	279.270425	6.308506
6.140478	281.074122	6.313510
5.961328	276.657227	6.318515
5.720022	262.347654	6.323520
5.660944	263.688969	6.328525
5.902785	278.698041	6.333530
6.329007	275.898450	6.338534
5.700626	269.732377	6.343539
5.833126	257.737377	6.348544
5.683520	267.125399	6.353549
5.528701	257.782016	6.358554
6.056522	267.241731	6.363558
5.612117	268.946756	6.368563
6.010253	275.152245	6.373568
5.772493	269.615039	6.378573
5.982207	275.343674	6.383578
5.873508	265.088291	6.388582
5.248535	266.688554	6.393587
5.895953	277.066106	6.398592
5.917017	279.771151	6.403597
5.691975	282.457568	6.408602
5.808477	274.157080	6.413606
5.950955	282.082298	6.418611
6.130664	282.861262	6.423616
6.229991	278.470610	6.428621
6.120328	268.857605	6.433626
5.558670	252.304241	6.438630
5.274265	257.733325	6.443635
5.386410	267.580456	6.448640
5.386991	277.593657	6.453645
5.740333	277.342696	6.458650
6.160389	276.796615	6.463654
5.971611	291.208368	6.468659
6.124271	273.408000	6.473664
5.649455	282.552441	6.478669
6.020961	279.416526	6.483674
6.268981	276.923086	6.488678
6.039693	282.311959	6.493683
5.839721	263.155497	6.498688
5.464829	263.470328	6.503693
5.781252	273.383732	6.508698
5.994567	282.414705	6.513702
5.879311	277.342468	6.518707
5.972945	266.327931	6.523712
5.630049	272.110969	6.528717
5.914031	272.085938	6.533722
5.700378	262.498618	6.538726
6.033863	269.802481	6.543731
6.251203	259.423573	6.548736
6.179323	261.070595	6.553741
5.746350	260.277686	6.558746
5.553613	251.734297	6.563750
5.486388	251.577291	6.568755
5.753258	254.259879	6.573760
5.673206	262.820837	6.578765
5.694799	270.685780	6.583770
6.009873	270.434449	6.588774
5.822361	270.520793	6.593779
5.579999	264.756520	6.598784
5.953933	277.989175	6.603789
5.792109	282.013483	6.608794
6.041337	281.389597	6.613798
5.856971	273.471306	6.618803
5.234656	265.681316	6.623808
5.993393	274.668492	6.628813
5.897622	281.007830	6.633818
5.873160	285.580217	6.638822
5.897998	282.023722	6.643827
6.256845	280.411515	6.648832
5.620381	274.332119	6.653837
5.481483	271.737574	6.658842
6.037646	283.470744	6.663846
5.841350	280.973717	6.668851
6.056615	287.391177	6.673856
5.764339	264.398869	6.678861
5.348781	271.224583	6.683866
5.803706	272.973078	6.688870
5.635892	290.693953	6.693875
6.038780	288.467459	6.698880
6.058699	276.739907	6.703885
5.842811	282.772087	6.708890
5.679491	280.355346	6.713894
6.004065	287.901045	6.718899
6.371216	283.187123	6.723904
5.595136	265.417473	6.728909
5.714442	265.873653	6.733914
5.993932	273.331455	6.738918
5.917433	273.498589	6.743923
5.823828	266.929721	6.748928
5.577045	268.717869	6.753933
5.492517	268.221877	6.758938
5.973353	284.180815	6.763942
5.920744	284.375866	6.768947
5.722637	293.863201	6.773952
6.115404	287.224926	6.778957
5.680846	285.742577	6.783962
6.144683	276.957746	6.788966
5.719700	270.690403	6.793971
5.549808	269.625583	6.798976
5.917549	277.879552	6.803981
5.831483	287.317801	6.808986
5.967714	282.225389	6.813990
6.294273	283.443389	6.818995
5.821845	270.229633	6.824000
5.756664	268.772031	6.829005
5.740432	272.963489	6.834010
5.874783	269.484857	6.839014
5.595599	263.185326	6.844019
5.672546	255.960333	6.849024
5.888483	264.035454	6.854029
5.652139	271.959539	6.859034
5.807210	282.780740	6.864038
6.017244	277.578764	6.869043
5.952342	273.846422	6.874048
5.870107	272.195326	6.879053
5.578291	257.286192	6.884058
5.982431	269.919365	6.889062
5.801396	277.635529	6.894067
5.941700	264.823076	6.899072
5.517702	267.091224	6.904077
5.819630	275.336455	6.909082
5.972987	279.295871	6.914086
5.952309	276.945505	6.919091
5.675108	271.395457	6.924096
5.513675	272.066187	6.929101
6.005196	284.233357	6.934106
6.267782	281.335859	6.939110
5.858602	283.123983	6.944115
5.917400	266.530950	6.949120
5.884339	264.290078	6.954125
5.790188	262.030246	6.959130
6.115102	262.894167	6.964134
5.734249	264.624096	6.969139
6.066186	256.372330	6.974144
5.712917	261.249000	6.979149
5.690782	254.093217	6.984154
5.755150	254.016960	6.989158
5.744365	259.963416	6.994163
5.473351	260.265237	6.999168
5.846980	259.527073	7.004173
6.057532	271.083096	7.009178
6.203337	261.420827	7.014182
5.759640	266.425471	7.019187
5.834361	264.936595	7.024192
6.193320	251.950905	7.029197
5.950260	264.086904	7.034202
5.365086	260.910124	7.039206
5.482832	263.843717	7.044211
5.686071	256.364947	7.049216
6.140121	257.721280	7.054221
5.852815	258.446408	7.059226
5.912735	256.333427	7.064230
5.889302	265.708131	7.069235
6.133440	253.613496	7.074240
5.666174	261.377382	7.079245
5.328725	261.629437	7.084250
5.713231	262.075963	7.089254
5.544397	262.327075	7.094259
5.845007	269.993554	7.099264
5.828826	271.938783	7.104269
5.970257	280.455774	7.109274
6.181997	279.774452	7.114278
5.845474	271.525518	7.119283
5.897437	264.959296	7.124288
6.023724	265.816178	7.129293
5.335399	267.631945	7.134298
5.733724	264.669024	7.139302
5.793434	271.977549	7.144307
6.215282	274.708776	7.149312
5.942503	265.674815	7.154317
5.647931	268.498603	7.159322
5.875894	264.527680	7.164326
5.747004	275.146320	7.169331
5.965465	258.234211	7.174336
5.957116	268.100104	7.179341
5.764906	269.867100	7.184346
5.981218	266.900880	7.189350
5.795873	267.799956	7.194355
6.085834	262.892418	7.199360
6.084473	270.786244	7.204365
5.546769	276.216807	7.209370
5.910377	262.505899	7.214374
5.397592	269.125292	7.219379
5.580084	268.410560	7.224384
5.628962	272.943051	7.229389
5.807023	283.235500	7.234394
6.121356	286.394748	7.239398
6.014990	277.050139	7.244403
5.888277	266.591919	7.249408
5.934861	267.780744	7.254413
5.953637	268.847351	7.259418
5.849863	262.248431	7.264422
5.528785	273.922031	7.269427
5.940665	267.859743	7.274432
5.464649	260.967611	7.279437
5.521336	268.105766	7.284442
6.397530	270.715632	7.289446
6.141139	276.712989	7.294451
6.264054	265.235158	7.299456
6.349227	265.997204	7.304461
6.081938	268.709179	7.309466
6.730619	261.129416	7.314470
5.902719	262.100062	7.319475
5.568754	251.095165	7.324480
6.055423	263.104891	7.329485
5.747520	248.641186	7.334490
5.809196	239.798769	7.339494
5.476094	249.364045	7.344499
5.748290	255.114582	7.349504
5.620760	259.155691	7.354509
5.677796	256.805882	7.359514
5.863729	261.430924	7.364518
5.829029	262.683024	7.369523
5.556991	258.169867	7.374528
5.742885	256.011963	7.379533
5.672607	268.178009	7.384538
5.924909	264.193804	7.389542
5.820193	255.620890	7.394547
5.714756	263.069018	7.399552
5.920365	259.427436	7.404557
5.476163	254.510824	7.409562
5.901637	263.492936	7.414566
5.686299	275.070981	7.419571
5.736206	273.902337	7.424576
5.583083	268.671487	7.429581
5.890791	269.000259	7.434586
5.841333	259.036206	7.439590
6.101955	267.139172	7.444595
5.886606	263.303708	7.449600
5.819818	261.843193	7.454605
5.591784	266.225812	7.459610
5.883629	260.549204	7.464614
6.028949	258.071756	7.469619
5.679401	262.795990	7.474624
5.420035	262.311403	7.479629
5.528291	267.717318	7.484634
5.470726	262.389335	7.489638
5.881486	285.578729	7.494643
5.828396	280.518958	7.499648
6.106346	284.838619	7.504653
5.906255	277.498567	7.509658
6.050369	261.784416	7.514662
6.042017	263.937229	7.519667
5.549850	263.833730	7.524672
5.954325	263.362840	7.529677
5.809917	266.213867	7.534682
6.015662	258.870745	7.539686
5.938735	265.254599	7.544691
5.687480	264.196120	7.549696
5.945696	262.963407	7.554701
5.886878	269.360262	7.559706
5.750768	262.475316	7.564710
5.790966	266.360601	7.569715
5.581022	266.934482	7.574720
5.642499	265.137627	7.579725
5.286337	267.439504	7.584730
5.727886	271.499577	7.589734
6.003306	284.310986	7.594739
6.130242	283.870654	7.599744
5.789878	273.657662	7.604749
5.810644	273.958346	7.609754
5.997952	273.258682	7.614758
5.716919	266.370990	7.619763
5.391883	262.590569	7.624768
5.656757	270.980771	7.629773
5.993991	284.076779	7.634778
6.274487	291.452175	7.639782
5.789840	280.382137	7.644787
5.717464	270.589321	7.649792
6.030583	274.245456	7.654797
6.094688	281.556466	7.659802
5.967113	267.248164	7.664806
5.849475	265.226101	7.669811
5.866993	265.590564	7.674816
5.943149	257.587425	7.679821
5.359724	259.488097	7.684826
5.880249	265.744128	7.689830
5.590680	273.568936	7.694835
5.924448	270.014963	7.699840
6.022842	275.849515	7.704845
5.577600	270.224392	7.709850
6.144004	267.475742	7.714854
5.874382	272.924674	7.719859
6.135211	265.392642	7.724864
5.919489	267.232900	7.729869
6.040688	269.691403	7.734874
5.782016	265.460896	7.739878
5.825896	266.482466	7.744883
5.584535	262.575125	7.749888
5.710837	265.118252	7.754893
5.497984	271.083518	7.759898
5.930001	264.622635	7.764902
5.863210	272.814545	7.769907
5.623374	272.073821	7.774912
5.812157	267.352874	7.779917
5.724182	268.176679	7.784922
5.983253	271.021832	7.789926
6.343948	273.000130	7.794931
6.336054	272.950942	7.799936
6.065690	262.303124	7.804941
5.931037	273.514271	7.809946
5.980711	259.089795	7.814950
5.736469	264.588556	7.819955
5.678495	265.866425	7.824960
5.657498	266.081864	7.829965
5.593390	274.055062	7.834970
5.620125	263.275566	7.839974
5.773298	276.820997	7.844979
5.983441	272.900301	7.849984
5.924103	264.472175	7.854989
5.718413	280.335523	7.859994
5.640191	263.368364	7.864998
5.463564	271.058529	7.870003
5.715758	276.938736	7.875008
5.972279	264.516305	7.880013
5.709368	270.476710	7.885018
5.967978	267.598816	7.890022
5.634043	267.037255	7.895027
5.615322	273.636671	7.900032
6.029115	270.608067	7.905037
6.046330	275.866810	7.910042
6.037601	266.981558	7.915046
5.916066	270.180194	7.920051
5.552329	269.411306	7.925056
5.987077	270.995267	7.930061
5.529531	271.326131	7.935066
5.680525	261.144209	7.940070
5.707975	262.013316	7.945075
5.818937	271.439863	7.950080
6.225637	273.164229	7.955085
5.898310	272.680732	7.960090
5.868555	263.827228	7.965094
6.241643	262.886672	7.970099
6.054994	260.606441	7.975104
5.824521	249.715142	7.980109
5.553249	255.891975	7.985114
5.857102	259.856428	7.990118
5.879401	259.832312	7.995136
5.974883	256.873455	8.000154
5.740511	250.507398	8.005171
5.793971	260.597260	8.010189
5.961006	256.093631	8.015206
5.718049	266.254892	8.020224
5.980339	260.919125	8.025242
6.149043	256.500438	8.030259
5.957970	256.981644	8.035277
5.945431	262.212662	8.040294
5.800263	262.623609	8.045312
5.709945	259.397052	8.050330
5.839548	255.984785	8.055347
5.677928	258.291664	8.060365
5.497641	257.944419	8.065382
5.587980	269.120388	8.070400
5.604735	259.174620	8.075418
6.373734	267.278640	8.080435
5.856871	269.694477	8.085453
5.711672	267.599865	8.090470
5.742272	279.144882	8.095488
5.856103	281.402567	8.100506
6.190812	283.909867	8.105523
6.221421	290.090329	8.110541
5.944517	272.345393	8.115558
6.002897	267.464226	8.120576
5.610065	269.873375	8.125594
6.047610	276.271323	8.130611
5.908350	287.959551	8.135629
5.999998	285.184313	8.140646
6.071382	289.578654	8.145664
6.091262	289.206554	8.150682
6.086554	276.209473	8.155699
6.081694	273.780603	8.160717
5.936110	263.475123	8.165734
5.752949	272.083979	8.170752
5.999253	281.184518	8.175770
6.598952	275.695233	8.180787
6.188303	270.754555	8.185805
5.974268	268.405588	8.190822
6.068178	259.823659	8.195840
5.869332	263.663656	8.200858
5.965917	259.354021	8.205875
6.195322	260.981518	8.210893
5.948222	260.183954	8.215910
6.069137	261.102550	8.220928
5.714258	257.743626	8.225946
6.186065	270.034092	8.230963
6.225203	283.322842	8.235981
5.802292	269.548328	8.240998
6.231137	281.586731	8.246016
6.143681	281.830911	8.251034
6.281553	281.980051	8.256051
5.949869	274.786585	8.261069
5.639137	275.942792	8.266086
6.141001	284.785804	8.271104
6.116608	289.561110	8.276122
6.317203	281.237099	8.281139
6.078312	292.246605	8.286157
6.004902	294.763804	8.291174
6.427102	292.293685	8.296192
6.440243	284.014637	8.301210
6.229540	279.276342	8.306227
6.087447	272.252162	8.311245
6.532200	277.494031	8.316262
6.051952	269.335989	8.321280
6.056215	262.345826	8.326298
5.887641	269.794297	8.331315
6.095195	283.902532	8.336333
5.949873	282.909250	8.341350
6.325703	281.440373	8.346368
6.215036	292.824368	8.351386
6.349520	290.982836	8.356403
6.452725	294.390825	8.361421
6.460076	277.803919	8.366438
6.241201	273.372993	8.371456
6.197507	277.618001	8.376474
5.862225	264.148566	8.381491
6.247469	268.869553	8.386509
6.350110	280.889321	8.391526
6.428530	278.482195	8.396544
5.841978	280.211492	8.401562
6.276141	287.815420	8.406579
6.243085	293.235823	8.411597
6.192086	292.846357	8.416614
6.161034	294.473387	8.421632
6.484594	302.599442	8.426650
6.228304	288.959908	8.431667
6.203039	289.276451	8.436685
6.254786	295.737630	8.441702
6.110884	294.043578	8.446720
6.279659	299.104373	8.451738
6.482764	293.029928	8.456755
6.252433	295.044570	8.461773
6.081492	294.396084	8.466790
6.338702	293.232837	8.471808
6.196892	294.195496	8.476826
6.576185	285.588055	8.481843
6.454590	289.318205	8.486861
6.496317	290.157619	8.491878
6.759875	294.474706	8.496896
6.747112	293.738479	8.501914
6.188123	281.184281	8.506931
6.662138	282.858897	8.511949
6.079976	277.944922	8.516966
6.636289	280.534477	8.521984
6.309973	274.580335	8.527002
6.141724	267.049019	8.532019
6.529416	270.725115	8.537037
6.536709	288.897420	8.542054
6.213096	279.888210	8.547072
5.977830	285.999620	8.552090
6.689544	283.793676	8.557107
6.342039	285.574112	8.562125
6.429822	289.461000	8.567143
6.359290	291.141510	8.572160
6.314774	294.250624	8.577178
6.325372	283.144532	8.582195
6.390507	292.124969	8.587213
6.478275	290.694631	8.592231
6.584950	288.232615	8.597248
6.536989	292.456201	8.602266
6.485816	291.558707	8.607283
6.311045	293.009309	8.612301
6.117174	285.614510	8.617319
6.397370	286.378927	8.622336
6.255353	289.683092	8.627354
6.410960	289.217280	8.632371
6.452423	292.082646	8.637389
6.221329	292.630041	8.642407
6.234667	288.876129	8.647424
6.159449	292.015268	8.652442
6.387572	307.754933	8.657459
6.561765	308.397008	8.662477
6.668169	305.834052	8.667495
6.864254	296.908011	8.672512
6.648624	301.596337	8.677530
6.349411	284.416564	8.682547
6.545225	297.627284	8.687565
6.310676	306.581810	8.692583
6.524482	303.055443	8.697600
6.466696	309.824000	8.702618
6.379806	311.074738	8.707635
6.587669	305.321422	8.712653
6.805257	319.036824	8.717671
6.874870	309.650812	8.722688
6.988900	318.140839	8.727706
7.280683	309.632213	8.732723
7.030856	296.108425	8.737741
6.520857	296.983251	8.742759
6.911246	286.499639	8.747776
6.266838	290.816091	8.752794
6.313213	283.642649	8.757811
6.392525	281.162805	8.762829
6.533690	293.116625	8.767847
6.415695	296.275048	8.772864
6.629590	304.118394	8.777882
6.796877	307.024129	8.782899
6.779959	306.045566	8.787917
6.730245	317.625202	8.792935
6.988916	307.338802	8.797952
6.928660	301.939640	8.802970
6.657659	295.481445	8.807987
6.764726	289.882675	8.813005
6.625450	284.707249	8.818023
6.587621	278.932238	8.823040
6.484658	295.865778	8.828058
6.723675	302.433494	8.833075
7.071003	302.158725	8.838093
6.323907	306.992913	8.843111
6.784886	308.436044	8.848128
6.751392	314.733787	8.853146
6.937714	305.446365	8.858163
6.562172	310.481465	8.863181
6.808413	314.148038	8.868199
6.862436	304.938015	8.873216
6.477580	316.197467	8.878234
6.592392	314.781850	8.883251
6.688282	311.863944	8.888269
6.600005	319.309400	8.893287
6.763802	306.743628	8.898304
6.680526	321.294783	8.903322
6.923957	307.703654	8.908339
6.835149	315.998056	8.913357
6.551529	320.876844	8.918375
6.585567	311.647840	8.923392
6.742363	319.926093	8.928410
6.763677	315.615542	8.933427
7.266233	307.042544	8.938445
6.817510	308.750383	8.943463
6.840135	306.093180	8.948480
6.771757	313.516602	8.953498
6.826456	316.853256	8.958515
6.615992	317.624645	8.963533
6.725597	322.132957	8.968551
7.068679	322.650912	8.973568
7.290707	325.563906	8.978586
7.183293	329.156164	8.983603
7.321722	311.728354	8.988621
7.141662	322.043946	8.993639
7.307279	315.890128	8.998656
7.603844	314.711286	9.003674
7.180449	315.373824	9.008691
7.272098	313.879767	9.013709
6.667079	305.280412	9.018727
6.947994	303.539149	9.023744
6.827174	305.290604	9.028762
6.983906	316.049189	9.033779
7.099534	308.082358	9.038797
7.259022	317.606664	9.043815
7.210223	306.613940	9.048832
7.096139	295.107555	9.053850
6.676668	292.841060	9.058867
6.812001	298.497164	9.063885
6.421397	314.838071	9.068903
6.960210	310.090361	9.073920
6.871006	311.906317	9.078938
6.791421	308.384607	9.083955
7.269723	304.908572	9.088973
7.077997	313.752298	9.093991
7.073525	305.842035	9.099008
7.283948	309.296445	9.104026
6.877144	316.551666	9.109043
7.045585	311.804821	9.114061
7.190312	313.000563	9.119079
7.146345	305.175341	9.124096
6.943961	307.961918	9.129114
6.795758	307.171044	9.134131
6.830370	300.214009	9.139149
6.952410	305.727026	9.144167
6.669344	308.642924	9.149184
7.023479	302.879457	9.154202
6.899975	319.835152	9.159219
7.835995	332.416282	9.164237
7.146749	322.479422	9.169255
6.848638	308.224725	9.174272
7.211977	311.854132	9.179290
6.928548	323.836214	9.184307
7.228815	326.159545	9.189325
7.279834	336.000535	9.194343
7.495429	326.544450	9.199360
7.183388	331.812653	9.204378
6.756201	317.177280	9.209395
7.096768	325.720397	9.214413
6.900862	332.658781	9.219431
7.431074	327.151899	9.224448
7.342298	331.318737	9.229466
7.193370	341.171926	9.234483
7.529174	337.001743	9.239501
7.415251	344.419646	9.244519
7.565816	322.392176	9.249536
7.219094	319.824033	9.254554
7.237874	314.807015	9.259571
6.974036	300.651124	9.264589
7.339592	323.368588	9.269607
7.253652	323.360082	9.274624
7.086568	325.901338	9.279642
7.568819	333.990077	9.284659
7.473899	319.864672	9.289677
7.041680	331.759478	9.294695
7.596533	328.508192	9.299712
8.008927	319.138229	9.304730
7.187614	309.452300	9.309747
7.279693	304.105154	9.314765
6.891401	307.482378	9.319783
6.985056	310.102950	9.324800
7.331760	321.769182	9.329818
7.399245	328.186899	9.334835
7.513035	322.615473	9.339853
7.519926	332.182480	9.344871
7.509630	330.574913	9.349888
7.312091	318.112727	9.354906
7.270291	325.838112	9.359923
7.171540	332.635144	9.364941
7.507053	326.909281	9.369959
7.550566	325.246003	9.374976
7.713517	328.272331	9.379994
7.357790	319.978118	9.385011
7.300740	322.707358	9.390029
7.411801	318.957157	9.395047
7.157659	326.892319	9.400064
7.303983	334.945004	9.405082
7.784058	329.423838	9.410099
7.809037	324.626746	9.415117
7.971906	325.037068	9.420135
7.459127	314.574147	9.425152
7.541252	304.971606	9.430170
6.837086	319.957084	9.435187
7.367726	317.015666	9.440205
7.915370	324.974306	9.445223
7.451740	319.499095	9.450240
7.743567	308.765743	9.455258
7.141956	328.203631	9.460275
7.760812	321.401762	9.465293
7.489132	321.431642	9.470311
7.577822	322.863315	9.475328
7.719986	321.702201	9.480346
7.488679	318.182022	9.485363
7.507577	320.842634	9.490381
7.743375	325.511171	9.495399
7.218101	320.152849	9.500416
7.707616	322.478271	9.505434
7.509857	327.135420	9.510451
7.791612	331.200388	9.515469
7.517780	321.634327	9.520487
7.475484	325.008174	9.525504
7.755698	326.167044	9.530522
7.718500	333.885405	9.535539
7.801025	328.615474	9.540557
7.722164	330.486623	9.545575
7.879901	324.908354	9.550592
7.728400	306.547444	9.555610
7.449488	308.853659	9.560627
7.357401	316.220816	9.565645
7.815992	325.225212	9.570663
7.774905	325.752492	9.575680
7.984204	316.486731	9.580698
7.486428	307.239551	9.585715
7.518940	316.244014	9.590733
7.770949	329.976155	9.595751
7.415988	337.043442	9.600768
7.989498	329.409231	9.605786
7.575844	327.053469	9.610803
7.896258	325.224008	9.615821
7.799598	333.396571	9.620839
7.329723	323.946234	9.625856
7.764341	324.229043	9.630874
7.521073	330.303846	9.635891
7.725006	334.336753	9.640909
7.680742	326.249649	9.645927
7.451682	336.411942	9.650944
7.888694	326.347058	9.655962
7.924764	340.639820	9.660979
8.008669	329.402370	9.665997
7.916240	338.735549	9.671015
7.534268	332.250440	9.676032
7.896270	329.145939	9.681050
7.713252	335.968716	9.686067
7.567291	328.553817	9.691085
7.587261	334.843243	9.696103
7.759867	330.534377	9.701120
7.706366	316.755956	9.706138
7.616661	329.197002	9.711155
7.912853	328.766102	9.716173
7.890685	331.657160	9.721191
7.850025	337.959182	9.726208
7.985273	329.673724	9.731226
8.148482	337.531288	9.736243
7.872306	330.941349	9.741261
8.118836	325.052626	9.746279
7.510813	328.015966	9.751296
7.942229	334.916636	9.756314
8.235848	334.501914	9.761331
7.977428	333.242231	9.766349
7.767757	332.855380	9.771367
7.681777	341.480695	9.776384
8.285360	348.547058	9.781402
8.023555	351.920375	9.786419
7.964215	348.752091	9.791437
8.107118	348.890982	9.796455
7.742812	345.565065	9.801472
7.984582	349.623640	9.806490
7.890332	358.537413	9.811507
8.159193	355.030865	9.816525
7.984099	350.069269	9.821543
8.071071	369.049714	9.826560
8.507912	349.707266	9.831578
7.944316	347.213910	9.836595
7.914906	344.700494	9.841613
8.107323	350.167856	9.846631
8.188255	350.650893	9.851648
8.178855	346.610190	9.856666
7.760177	338.477240	9.861683
7.823472	350.282286	9.866701
8.259974	358.132020	9.871719
8.035451	364.566815	9.876736
8.766181	354.920063	9.881754
8.066799	344.719695	9.886771
7.647954	340.341977	9.891789
7.923422	352.918677	9.896807
8.009410	350.986864	9.901824
8.116645	351.039795	9.906842
7.892115	357.061200	9.911859
7.780573	354.797244	9.916877
8.096658	352.643423	9.921895
7.850693	352.350581	9.926912
7.865345	356.018508	9.931930
7.907209	358.082291	9.936947
8.144037	366.679447	9.941965
8.279189	362.007195	9.946983
8.223898	378.324353	9.952000
8.521452	374.743910	9.957018
8.159632	364.304790	9.962035
8.090757	368.872459	9.967053
8.562043	359.546952	9.972071
8.149388	369.946121	9.977088
8.091821	355.960030	9.982106
8.379186	361.851246	9.987123
8.150834	362.470796	9.992141
9.010803	361.223163	9.997159
8.288753	365.135176	10.002176
8.543389	358.431025	10.007194
8.524623	364.568710	10.012211
8.363386	359.049561	10.017229
8.148775	356.779563	10.022247
8.084483	363.299857	10.027264
8.216965	364.181945	10.032282
8.068412	360.238640	10.037299
8.069532	366.379541	10.042317
8.350643	374.941406	10.047335
8.518739	383.931104	10.052352
8.424444	379.676405	10.057370
8.444681	381.797204	10.062387
8.209547	382.294740	10.067405
8.746608	376.139870	10.072423
8.330657	377.306154	10.077440
8.324534	366.925255	10.082458
8.506031	378.408974	10.087475
8.144902	379.418408	10.092493
8.553219	372.857572	10.097511
8.433339	383.419437	10.102528
8.778364	381.339999	10.107546
8.394879	377.449046	10.112563
8.225723	368.093868	10.117581
8.577208	376.616375	10.122599
8.753629	383.925977	10.127616
8.577219	377.531915	10.132634
8.203017	368.975483	10.137651
8.519268	378.895114	10.142669
9.021032	369.773128	10.147687
8.304010	376.675907	10.152704
8.570249	369.648070	10.157722
8.643860	369.374894	10.162739
8.019876	376.458837	10.167757
8.419053	370.429573	10.172775
8.317167	389.054457	10.177792
8.546233	393.717748	10.182810
8.837357	388.027177	10.187827
8.588621	388.785595	10.192845
9.181210	391.328495	10.197863
9.167896	378.222233	10.202880
8.855239	371.243504	10.207898
8.462389	366.836487	10.212915
8.458284	376.370517	10.217933
8.929570	358.278642	10.222951
8.505193	355.981347	10.227968
8.629030	360.039353	10.232986
8.525115	358.130796	10.238003
8.594680	368.303413	10.243021
8.753822	355.640507	10.248039
8.227697	352.191468	10.253056
8.696518	365.331332	10.258074
8.879616	379.601233	10.263091
8.668936	371.820871	10.268109
8.822088	360.231812	10.273127
8.487719	369.735214	10.278144
8.503776	375.725477	10.283162
8.935444	384.263905	10.288179
8.976389	386.668644	10.293197
8.660546	379.220217	10.298215
8.841782	380.533349	10.303232
8.854165	382.753196	10.308250
8.923929	380.123354	10.313267
8.368238	374.861265	10.318285
8.738370	373.462692	10.323303
9.130497	383.032859	10.328320
9.181863	380.418504	10.333338
9.021286	367.805369	10.338355
8.590400	365.266101	10.343373
8.477486	360.613540	10.348391
8.572313	378.854354	10.353408
9.057670	383.515606	10.358426
9.137967	375.860344	10.363443
8.704267	385.363441	10.368461
8.694401	381.827705	10.373479
9.041636	390.726402	10.378496
9.127298	389.233271	10.383514
9.041700	382.124516	10.388531
8.761140	372.325958	10.393549
8.702675	368.046749	10.398567
8.789480	380.734890	10.403584
9.127291	380.467912	10.408602
9.056991	379.115824	10.413619
9.014315	389.877100	10.418637
8.756038	374.003614	10.423655
9.045673	376.426433	10.428672
8.710771	383.787245	10.433690
9.305406	382.451541	10.438707
9.183313	386.532066	10.443725
8.936373	379.634615	10.448743
8.716208	376.923690	10.453760
8.866554	380.141328	10.458778
9.069439	385.417732	10.463795
8.953030	393.097961	10.468813
9.277009	384.142496	10.473831
9.393906	393.528315	10.478848
8.594172	388.149592	10.483866
9.142481	386.230996	10.488883
9.158782	388.311385	10.493901
9.342190	386.992374	10.498919
9.246367	388.787279	10.503936
8.810503	381.019885	10.508954
9.106758	381.964833	10.513971
8.519323	385.660242	10.518989
8.614215	388.801313	10.524007
8.964985	393.836955	10.529024
8.995216	395.429207	10.534042
9.238809	390.285651	10.539059
9.039834	399.509225	10.544077
9.080379	401.645799	10.549095
8.788645	396.658170	10.554112
9.022861	394.229928	10.559130
8.897728	385.145583	10.564147
9.055881	394.988858	10.569165
9.101191	408.765866	10.574183
9.468943	414.265905	10.579200
9.250678	408.395876	10.584218
9.116438	396.996698	10.589235
9.545380	406.286604	10.594253
9.363202	393.676814	10.599271
9.487280	389.984529	10.604288
9.229738	389.747134	10.609306
9.228738	385.585199	10.614323
9.472636	398.649660	10.619341
9.304996	389.682379	10.624359
9.537996	387.121790	10.629376
8.880749	385.239425	10.634394
9.081998	374.542226	10.639411
9.078183	397.607615	10.644429
9.449538	399.752638	10.649447
9.727670	398.239006	10.654464
9.338933	398.861440	10.659482
9.325315	378.879075	10.664499
9.203939	392.644155	10.669517
9.498637	384.728300	10.674535
9.258522	389.625578	10.679552
9.263016	390.300389	10.684570
9.252093	399.570420	10.689587
9.296564	413.527433	10.694605
9.382537	417.187424	10.699623
9.571627	411.989235	10.704640
9.279432	416.048916	10.709658
9.979479	408.328702	10.714675
9.164818	414.836464	10.719693
9.506361	406.465204	10.724711
9.707625	415.197303	10.729728
9.788524	412.751905	10.734746
9.570593	398.301624	10.739763
9.293697	391.437234	10.744781
9.744889	385.952104	10.749799
9.734841	385.559416	10.754816
9.386123	389.328105	10.759834
9.357235	393.255271	10.764851
9.111906	394.467571	10.769869
9.287008	403.345740	10.774887
9.448831	404.781812	10.779904
9.625832	409.434279	10.784922
10.013391	409.112222	10.789939
9.673675	405.997049	10.794957
9.565828	399.333541	10.799975
9.843289	397.450803	10.804992
9.433469	398.325815	10.810010
9.562233	388.040660	10.815027
9.385811	395.354713	10.820045
9.466117	405.642438	10.825063
9.761013	404.602698	10.830080
9.496386	409.125120	10.835098
9.483481	406.962559	10.840115
9.601580	400.257561	10.845133
9.595589	409.927596	10.850151
9.697860	404.941732	10.855168
9.467083	410.623318	10.860186
9.430195	402.109020	10.865203
9.596289	415.532728	10.870221
9.583959	414.143210	10.875239
9.987054	412.259843	10.880256
9.419907	417.072354	10.885274
9.250363	411.914226	10.890291
9.588552	412.817935	10.895309
9.505300	413.206622	10.900327
9.982227	418.692820	10.905344
9.639959	427.096160	10.910362
9.908352	427.524767	10.915379
9.996362	432.670755	10.920397
9.652648	422.582215	10.925415
9.983520	418.232908	10.930432
9.755839	414.942508	10.935450
10.158688	420.392905	10.940467
9.772752	411.989750	10.945485
9.517055	405.709004	10.950503
9.824213	414.358346	10.955520
10.130205	424.273289	10.960538
10.048106	431.976593	10.965555
10.271119	417.956235	10.970573
9.547525	415.112258	10.975591
10.175069	405.487856	10.980608
9.681325	405.700626	10.985626
9.900991	410.775619	10.990643
9.766070	407.581225	10.995661
10.080765	420.615745	11.000679
10.384082	430.534264	11.005696
9.963707	417.232588	11.010714
9.455806	417.106753	11.015731
10.133310	424.319419	11.020749
10.001076	424.516927	11.025767
10.386751	427.107827	11.030784
9.683555	423.670566	11.035802
10.075883	420.223673	11.040819
10.157726	418.245164	11.045837
9.755465	411.485488	11.050855
10.277121	426.311753	11.055872
10.602282	429.322309	11.060890
9.961125	405.947472	11.065907
9.496046	407.424349	11.070925
9.903510	411.128953	11.075943
10.474877	425.543555	11.080960
10.350043	421.845840	11.085978
9.816115	409.189824	11.090995
10.136195	421.507175	11.096013
10.020286	433.961841	11.101031
10.683682	420.425153	11.106048
10.000391	416.094901	11.111066
9.878682	416.413840	11.116083
10.004370	416.984580	11.121101
10.158035	434.951216	11.126119
10.270995	431.042914	11.131136
10.143939	442.694631	11.136154
10.475237	433.646488	11.141171
10.196970	445.987593	11.146189
9.933685	434.567460	11.151207
10.468737	436.929987	11.156224
10.175009	439.563557	11.161242
9.956346	436.413752	11.166259
10.370630	444.014531	11.171277
10.013997	440.087828	11.176295
10.710668	430.143396	11.181312
10.026582	441.515785	11.186330
10.264582	435.798758	11.191347
10.323151	441.233341	11.196365
10.221266	437.828681	11.201383
10.113193	434.611168	11.206400
10.549770	445.742806	11.211418
10.449641	437.970449	11.216435
10.249551	447.711748	11.221453
10.333388	436.398506	11.226471
10.344202	432.130585	11.231488
10.367814	434.560119	11.236506
10.394742	441.476473	11.241523
10.709188	435.766478	11.246541
10.371437	441.335348	11.251559
10.632952	435.419009	11.256576
10.520130	438.491449	11.261594
10.234552	439.580637	11.266611
10.473901	435.015213	11.271629
10.155946	443.761898	11.276647
10.604707	437.153719	11.281664
10.418715	439.227742	11.286682
10.367513	442.662956	11.291699
10.508052	443.042045	11.296717
10.486176	446.419047	11.301735
10.262931	437.034386	11.306752
10.131754	435.117443	11.311770
10.436749	442.107263	11.316787
10.422751	439.563033	11.321805
10.535655	442.395212	11.326823
10.758651	437.175958	11.331840
10.668882	439.692570	11.336858
10.668680	437.998219	11.341875
10.604152	430.447529	11.346893
10.337770	439.975094	11.351911
10.701047	436.255024	11.356928
10.330518	441.087419	11.361946
10.911275	447.844966	11.366963
10.621947	439.966373	11.371981
10.309722	437.680006	11.376999
10.519609	447.344850	11.382016
10.705992	455.047386	11.387034
10.570998	459.268785	11.392051
10.892935	463.810342	11.397069
10.695848	469.256338	11.402087
10.874732	467.792865	11.407104
10.627238	464.136328	11.412122
10.682893	459.359669	11.417139
11.012734	457.718067	11.422157
10.803140	463.585710	11.427175
10.899232	460.266980	11.432192
10.703168	464.949147	11.437210
10.902899	462.207543	11.442227
10.569038	455.292040	11.447245
10.749174	464.368263	11.452263
10.703662	462.624163	11.457280
10.713982	468.542771	11.462298
10.700769	469.561153	11.467315
11.057079	466.517472	11.472333
10.733962	462.916889	11.477351
10.855644	461.023686	11.482368
10.913062	468.332917	11.487386
10.744020	461.312858	11.492403
11.368183	456.747472	11.497421
10.965865	469.985180	11.502439
10.803089	454.923535	11.507456
10.779213	462.939664	11.512474
11.002988	464.930957	11.517491
11.038992	471.659727	11.522509
10.910849	460.679262	11.527527
11.030908	460.108532	11.532544
11.058863	461.761102	11.537562
11.036332	458.321993	11.542579
11.134785	462.043163	11.547597
10.762036	464.685884	11.552615
10.885924	460.946280	11.557632
11.063447	457.501268	11.562650
11.059008	454.870345	11.567667
11.277528	458.178364	11.572685
10.955756	459.800183	11.577703
11.366270	459.761715	11.582720
11.458476	458.015107	11.587738
10.590718	462.498911	11.592755
11.141404	453.912038	11.597773
10.895344	468.128913	11.602791
11.026823	460.970550	11.607808
11.108096	463.766633	11.612826
11.095015	463.879321	11.617843
11.210579	460.109456	11.622861
10.870529	458.726780	11.627879
10.776831	465.892288	11.632896
10.885631	460.892770	11.637914
10.542272	468.911310	11.642931
11.081742	470.780871	11.647949
11.019081	483.019007	11.652967
11.215834	483.881628	11.657984
11.690877	481.384321	11.663002
11.206961	494.009931	11.668019
11.444997	482.022585	11.673037
11.096109	484.200868	11.678055
11.561026	477.788965	11.683072
11.469579	478.314623	11.688090
11.125266	471.343939	11.693107
11.040808	469.864666	11.698125
10.949809	479.544818	11.703143
11.321388	481.248025	11.708160
11.533593	486.065437	11.713178
11.246413	485.009028	11.718195
11.332900	485.718411	11.723213
11.125777	488.994882	11.728231
11.304665	480.039870	11.733248
11.319960	484.559752	11.738266
11.137287	487.908151	11.743283
11.270345	481.866638	11.748301
11.480152	487.201952	11.753319
11.413932	489.238399	11.758336
11.247308	488.286290	11.763354
11.250663	492.094854	11.768371
11.157267	483.046541	11.773389
11.435465	495.089610	11.778407
11.037201	494.444954	11.783424
11.551338	501.648376	11.788442
11.756854	511.717860	11.793459
11.821435	502.777479	11.798477
11.383767	491.337125	11.803495
11.521125	486.105946	11.808512
11.455126	492.831671	11.813530
11.365888	506.686505	11.818547
11.506707	508.005940	11.823565
11.510663	511.896461	11.828583
11.537429	511.223496	11.833600
11.439991	507.477318	11.838618
11.498648	513.593533	11.843635
11.820548	503.884128	11.848653
11.594054	512.970041	11.853671
11.509597	511.276179	11.858688
11.980409	510.398383	11.863706
11.748976	504.981632	11.868723
11.812678	513.624748	11.873741
11.830202	510.479180	11.878759
11.729076	510.902209	11.883776
11.851988	509.756703	11.888794
11.717253	520.087442	11.893811
12.024485	508.493231	11.898829
11.813126	512.114332	11.903847
11.759495	518.910722	11.908864
11.786585	500.695367	11.913882
11.567544	514.762913	11.918899
11.697693	512.830519	11.923917
11.505046	513.031122	11.928935
11.855025	509.606584	11.933952
11.847785	499.961051	11.938970
11.696264	514.352583	11.943987
11.899167	500.351070	11.949005
12.012968	504.170841	11.954023
11.725894	509.744464	11.959040
11.850657	506.822030	11.964058
11.832777	506.055035	11.969075
12.008739	505.305194	11.974093
11.980054	504.978519	11.979111
12.048203	510.499990	11.984128
11.902903	509.882216	11.989146
11.572050	511.060504	11.994163
11.646139	514.539337	11.999181
11.670736	508.795556	12.004199
11.897635	518.012841	12.009216
11.971882	517.326172	12.014234
11.936576	517.196178	12.019251
11.834481	512.286283	12.024269
11.688858	511.245700	12.029287
11.811916	530.766630	12.034304
12.233705	534.484808	12.039322
12.089919	537.896587	12.044339
12.180341	536.295410	12.049357
12.388493	534.464472	12.054375
12.066256	537.014137	12.059392
12.170872	536.748753	12.064410
12.191630	535.477145	12.069427
11.822171	525.761768	12.074445
12.102342	528.943441	12.079463
12.113366	526.180718	12.084480
12.353152	531.864813	12.089498
11.991149	534.824594	12.094515
11.987258	529.173601	12.099533
12.144870	542.671306	12.104551
11.937489	543.896641	12.109568
12.088361	536.230321	12.114586
11.934870	539.378535	12.119603
12.427444	535.180741	12.124621
12.045828	537.162163	12.129639
12.284512	539.488800	12.134656
12.424974	525.913537	12.139674
12.237493	541.655005	12.144691
12.292147	539.737518	12.149709
12.433754	531.996906	12.154727
12.165346	533.812385	12.159744
12.397125	537.118354	12.164762
12.127976	533.572468	12.169779
12.225528	532.894791	12.174797
12.698471	530.751240	12.179815
12.441552	538.027393	12.184832
12.416173	525.954804	12.189850
12.376347	533.582146	12.194867
12.602006	532.663627	12.199885
12.621223	524.421390	12.204903
12.472637	538.503230	12.209920
12.368253	537.954820	12.214938
12.131186	538.032957	12.219955
11.958366	534.932800	12.224973
12.167445	530.605585	12.229991
12.165417	537.482305	12.235008
12.575919	546.667864	12.240026
12.690583	550.900903	12.245043
12.753697	547.887080	12.250061
13.042131	540.959857	12.255079
12.514352	535.453543	12.260096
12.575481	532.989118	12.265114
12.629778	540.769059	12.270131
12.327593	538.070878	12.275149
12.333837	535.245785	12.280167
12.254431	556.167826	12.285184
13.146781	556.694939	12.290202
12.525270	565.864472	12.295219
12.511858	564.500356	12.300237
12.758190	551.747999	12.305255
12.526909	550.089616	12.310272
12.632838	564.308566	12.315290
12.981696	559.281111	12.320307
12.864520	558.870386	12.325325
13.146408	557.337222	12.330343
12.906793	551.603008	12.335360
12.891837	527.666628	12.340378
12.374141	535.352596	12.345395
12.460570	533.398606	12.350413
13.061921	544.100726	12.355431
12.799579	549.178225	12.360448
13.080011	551.198575	12.365466
12.773453	538.639604	12.370483
13.013252	533.821632	12.375501
12.717322	528.020457	12.380519
12.404417	543.554247	12.385536
12.777262	556.844890	12.390554
13.026510	554.726697	12.395571
12.922207	570.269055	12.400589
13.036026	563.788715	12.405607
13.021666	560.900556	12.410624
12.971236	569.419465	12.415642
12.936415	568.102861	12.420659
12.903661	567.360269	12.425677
13.184533	567.644931	12.430695
12.829502	564.355396	12.435712
12.735650	560.065873	12.440730
13.032759	559.098360	12.445747
12.726388	566.909222	12.450765
13.227793	551.680970	12.455783
12.966610	567.699013	12.460800
13.151893	563.706840	12.465818
12.889023	565.562484	12.470835
13.118131	566.088726	12.475853
13.386955	564.166291	12.480871
13.072493	563.565386	12.485888
13.145400	562.351926	12.490906
13.237815	567.459400	12.495923
13.213495	575.936378	12.500941
13.195705	570.069794	12.505959
13.039880	571.040961	12.510976
12.881544	567.411544	12.515994
13.111696	566.489169	12.521011
12.962782	568.607925	12.526029
13.429786	569.365359	12.531047
13.123732	579.748053	12.536064
13.142340	570.373001	12.541082
13.372310	574.947840	12.546099
13.306616	574.219843	12.551117
13.669975	560.720297	12.556135
13.138903	554.526553	12.561152
13.232070	567.964887	12.566170
13.476306	563.042079	12.571187
13.094241	555.865810	12.576205
13.616293	567.564860	12.581223
13.005728	567.669594	12.586240
13.439420	563.411536	12.591258
13.196636	566.579969	12.596275
13.070738	563.724954	12.601293
13.301784	554.600845	12.606311
13.259223	563.847486	12.611328
13.167653	560.980816	12.616346
13.428388	554.281953	12.621363
13.075004	557.748459	12.626381
13.491131	566.592339	12.631399
13.651797	571.417799	12.636416
13.356022	574.288383	12.641434
13.791410	571.557407	12.646451
13.396310	573.771297	12.651469
13.705620	558.453032	12.656487
13.252100	562.244386	12.661504
13.447543	579.204315	12.666522
13.485028	574.417832	12.671539
13.595781	595.666903	12.676557
13.906513	583.709195	12.681575
13.995721	591.808757	12.686592
13.243995	582.758757	12.691610
13.460023	573.091044	12.696627
13.512407	577.425301	12.701645
14.143859	579.255307	12.706663
13.748986	585.290688	12.711680
13.468009	570.966843	12.716698
13.839959	580.063751	12.721715
13.572308	591.907862	12.726733
13.934039	578.244461	12.731751
13.806131	580.905881	12.736768
13.565253	575.771434	12.741786
13.753921	593.666511	12.746803
13.672056	591.704005	12.751821
13.750153	589.520942	12.756839
13.987488	597.758383	12.761856
13.822972	594.726347	12.766874
14.063433	596.282729	12.771891
13.840557	588.933344	12.776909
13.793703	585.166651	12.781927
13.843424	576.436821	12.786944
13.900569	588.142001	12.791962
13.865809	584.995093	12.796979
13.882580	592.339105	12.801997
14.046079	596.416234	12.807015
13.858964	587.899992	12.812032
13.580077	591.421174	12.817050
14.138334	590.589718	12.822067
14.000468	584.726046	12.827085
13.961378	585.959894	12.832103
13.746390	586.356473	12.837120
13.931410	596.577514	12.842138
14.091562	593.450749	12.847155
14.018956	596.065692	12.852173
14.259732	597.423217	12.857191
13.880997	595.345993	12.862208
13.624065	595.802749	12.867226
14.198418	595.069768	12.872243
13.961743	593.932908	12.877261
13.934384	595.871802	12.882279
13.835396	599.286084	12.887296
13.914704	587.837757	12.892314
14.039178	587.420965	12.897331
13.807864	602.292032	12.902349
14.377333	588.018790	12.907367
14.271322	597.994822	12.912384
13.930474	604.400480	12.917402
14.212467	601.377814	12.922419
14.438636	610.563705	12.927437
14.499594	604.378747	12.932455
14.345598	595.917302	12.937472
13.947279	594.300701	12.942490
14.376449	595.669917	12.947507
14.326894	599.016545	12.952525
14.352408	590.369369	12.957543
14.155274	594.619408	12.962560
14.165177	611.636657	12.967578
14.529409	614.357151	12.972595
14.393053	625.360365	12.977613
14.527593	611.441989	12.982631
14.602110	607.864669	12.987648
14.221244	608.552152	12.992666
14.744048	603.141010	12.997683
14.608561	603.850246	13.002701
14.431980	590.945965	13.007719
14.486775	598.583848	13.012736
14.211593	597.260487	13.017754
14.242320	600.215934	13.022771
14.312731	617.466755	13.027789
14.349770	613.784820	13.032807
14.691092	609.935594	13.037824
14.466204	619.867033	13.042842
14.469846	613.690997	13.047859
14.640402	621.620123	13.052877
14.313232	619.487532	13.057895
14.441296	621.727265	13.062912
14.124674	622.022909	13.067930
14.440908	617.451780	13.072947
14.555715	621.186216	13.077965
14.726703	620.339318	13.082983
14.563557	616.060570	13.088000
14.350422	630.499658	13.093018
14.531697	626.186216	13.098035
14.605310	644.304377	13.103053
14.877120	637.698430	13.108071
14.953533	648.507590	13.113088
14.576821	640.670914	13.118106
14.659122	639.061525	13.123123
14.879018	652.454945	13.128141
14.966138	650.188421	13.133159
15.130842	645.656656	13.138176
14.449447	642.638819	13.143194
14.934646	635.239128	13.148211
14.600575	644.767874	13.153229
14.830127	648.686415	13.158247
15.090070	649.346708	13.163264
14.966512	654.213288	13.168282
15.220200	652.416273	13.173299
14.758469	636.908733	13.178317
14.978204	629.667136	13.183335
15.016610	627.957289	13.188352
14.786022	639.448535	13.193370
15.067515	639.780437	13.198387
15.037482	649.845651	13.203405
15.213330	652.109505	13.208423
14.948619	641.819198	13.213440
14.880065	648.946152	13.218458
15.153005	640.935746	13.223475
15.059635	643.165779	13.228493
15.005843	642.795675	13.233511
15.277365	644.678572	13.238528
14.986206	653.493768	13.243546
15.449913	639.681904	13.248563
14.724220	633.729865	13.253581
15.005422	646.192275	13.258599
15.142695	646.480363	13.263616
14.722866	655.378707	13.268634
14.871709	648.779278	13.273651
15.009174	658.736370	13.278669
14.802040	650.693412	13.283687
14.892634	651.531545	13.288704
15.124078	660.432628	13.293722
15.629424	664.494417	13.298739
15.252583	660.763308	13.303757
15.164429	651.064021	13.308775
15.085975	657.889574	13.313792
15.233498	662.701327	13.318810
15.487913	668.645110	13.323827
15.381551	677.611420	13.328845
15.322205	675.733758	13.333863
15.350150	676.767833	13.338880
15.221280	678.997087	13.343898
15.674095	683.335293	13.348915
15.656848	683.653751	13.353933
15.107692	676.620209	13.358951
15.631223	666.765718	13.363968
15.693217	670.486297	13.368986
15.898015	669.810852	13.374003
15.193946	649.904128	13.379021
15.434339	665.929368	13.384039
15.739001	670.180189	13.389056
15.268150	674.621182	13.394074
15.721130	685.258129	13.399091
15.575833	672.440434	13.404109
15.802682	682.623455	13.409127
15.695519	674.157836	13.414144
15.187279	673.826931	13.419162
15.752111	659.210383	13.424179
15.492838	667.553579	13.429197
15.496830	672.867347	13.434215
15.690459	679.347600	13.439232
15.443980	677.069899	13.444250
15.721493	672.104012	13.449267
15.571467	674.519589	13.454285
15.612843	682.478322	13.459303
15.688746	676.130073	13.464320
15.585288	678.860281	13.469338
15.766832	676.790483	13.474355
15.646053	672.890120	13.479373
15.379716	685.523012	13.484391
15.506196	673.183691	13.489408
15.840746	682.453726	13.494426
15.647862	675.421516	13.499443
15.955754	693.313909	13.504461
15.926109	696.827863	13.509479
15.829381	693.583291	13.514496
15.776406	700.348091	13.519514
15.598875	692.546649	13.524531
15.875472	696.044479	13.529549
15.667125	707.106287	13.534567
15.817824	695.085061	13.539584
15.764811	699.574609	13.544602
15.815188	708.563866	13.549619
15.938768	694.969013	13.554637
16.082498	700.308368	13.559655
16.369266	691.162890	13.564672
16.068282	692.895098	13.569690
15.817444	705.323626	13.574707
16.272629	695.514473	13.579725
16.340863	694.453205	13.584743
16.461319	691.383094	13.589760
16.034712	694.797913	13.594778
16.157774	706.189960	13.599795
16.115378	699.279473	13.604813
15.846306	705.620344	13.609831
16.092577	696.418055	13.614848
16.005267	705.987307	13.619866
16.022032	691.957822	13.624883
16.436995	702.073697	13.629901
15.866467	709.338789	13.634919
16.223180	711.707030	13.639936
16.154482	718.054577	13.644954
16.416162	721.873460	13.649971
16.502176	719.256817	13.654989
16.558436	724.180622	13.660007
16.454749	709.832217	13.665024
16.439343	731.060069	13.670042
16.525340	730.614551	13.675059
16.588025	723.116511	13.680077
16.220681	711.936456	13.685095
16.201849	719.058852	13.690112
16.751673	730.188816	13.695130
16.610346	718.411851	13.700147
16.472388	713.583222	13.705165
16.381924	723.042524	13.710183
16.912804	711.113568	13.715200
16.627827	708.845013	13.720218
16.220001	699.290143	13.725235
16.463318	707.971658	13.730253
16.176013	724.902750	13.735271
16.381809	724.369154	13.740288
16.496118	715.203180	13.745306
16.307855	717.104026	13.750323
16.414031	709.018571	13.755341
16.302541	723.321992	13.760359
16.415671	716.084335	13.765376
16.325139	728.459519	13.770394
16.373527	741.002424	13.775411
16.696691	749.523209	13.780429
16.695707	744.689023	13.785447
16.721231	751.419530	13.790464
16.993867	739.959939	13.795482
16.754979	749.656952	13.800499
16.882593	751.944108	13.805517
16.960892	747.435237	13.810535
16.748822	741.134957	13.815552
16.922745	749.817830	13.820570
17.012241	751.782727	13.825587
17.333671	741.748229	13.830605
16.993077	750.201951	13.835623
16.758129	726.356360	13.840640
16.821753	734.302185	13.845658
16.947123	746.211435	13.850675
17.043009	737.108276	13.855693
17.101705	746.355025	13.860711
16.979658	740.712894	13.865728
16.605391	754.924713	13.870746
16.807039	748.361206	13.875763
16.997308	753.649151	13.880781
16.931684	750.424972	13.885799
17.115357	743.886355	13.890816
17.056483	747.477451	13.895834
17.232539	745.907102	13.900851
17.128024	740.271708	13.905869
17.310755	753.794064	13.910887
17.460570	752.098416	13.915904
17.271556	750.367163	13.920922
16.824053	753.015254	13.925939
17.006182	745.927784	13.930957
17.177229	752.023426	13.935975
17.202882	746.093218	13.940992
17.152961	743.327327	13.946010
16.985830	736.537229	13.951027
17.289871	739.680511	13.956045
17.286506	749.230404	13.961063
16.997950	740.433246	13.966080
17.217540	741.611050	13.971098
16.975051	746.108021	13.976115
17.457891	752.420198	13.981133
17.437700	768.034836	13.986151
17.620883	769.533881	13.991168
17.289315	769.771895	13.996186
17.621238	775.533239	14.001203
17.577310	766.126796	14.006221
17.467642	764.594620	14.011239
17.954415	767.961913	14.016256
17.779329	756.764519	14.021274
17.064374	753.912829	14.026291
17.298741	755.050465	14.031309
17.748372	769.828273	14.036327
17.601273	777.718567	14.041344
17.653587	772.358538	14.046362
17.629254	780.860861	14.051379
17.741222	769.533561	14.056397
17.593047	777.651234	14.061415
17.693986	788.810100	14.066432
18.044719	782.188656	14.071450
17.658413	771.929828	14.076467
17.496365	764.596145	14.081485
17.705362	777.981890	14.086503
17.886768	779.184576	14.091520
17.527464	778.436015	14.096538
17.655086	776.645993	14.101555
17.692090	787.578135	14.106573
18.027651	785.850408	14.111591
18.163222	784.630331	14.116608
18.177329	789.175721	14.121626
17.968235	771.788947	14.126643
17.902862	758.438053	14.131661
17.333005	771.197156	14.136679
17.786210	776.046549	14.141696
18.194267	777.955539	14.146714
17.744310	792.778759	14.151731
18.191374	779.332286	14.156749
18.138053	788.924691	14.161767
18.102525	787.526133	14.166784
18.118524	783.582359	14.171802
17.563633	782.659129	14.176819
17.951676	779.045582	14.181837
18.199209	782.721518	14.186855
18.231231	782.659933	14.191872
17.953573	786.919399	14.196890
17.837746	782.948814	14.201907
17.858746	777.558947	14.206925
17.883825	778.978471	14.211943
18.067402	787.603056	14.216960
17.671973	781.476473	14.221978
17.649129	790.849546	14.226995
18.041884	794.919428	14.232013
17.829822	799.720935	14.237031
17.944710	796.667451	14.242048
18.105259	804.086991	14.247066
18.222882	807.110991	14.252083
18.543571	812.249264	14.257101
18.502968	818.646119	14.262119
18.637452	814.040123	14.267136
18.548570	811.352870	14.272154
18.225980	815.016597	14.277171
18.773834	803.151207	14.282189
18.747345	806.128219	14.287207
18.487673	804.783493	14.292224
18.595752	801.021033	14.297242
18.452868	807.108770	14.302259
18.597145	803.233379	14.307277
18.357462	807.887713	14.312295
18.537857	811.542552	14.317312
18.748779	803.970906	14.322330
18.376462	810.425716	14.327347
18.691850	799.006767	14.332365
18.555116	806.482061	14.337383
18.648963	811.295900	14.342400
18.738084	802.250565	14.347418
18.494041	804.078056	14.352435
18.552707	812.958780	14.357453
18.298952	798.068796	14.362471
17.976773	792.356825	14.367488
18.475351	796.710025	14.372506
18.256755	808.376233	14.377523
18.504087	804.970777	14.382541
18.716930	820.287253	14.387559
18.433014	829.577922	14.392576
18.806747	830.207883	14.397594
18.634529	830.168629	14.402611
18.963011	827.419547	14.407629
18.830821	831.580638	14.412647
18.695294	834.716639	14.417664
18.847961	833.522299	14.422682
18.947071	833.797398	14.427699
18.948360	820.994641	14.432717
18.925935	833.592817	14.437735
18.766855	829.303917	14.442752
19.469626	831.167026	14.447770
18.974399	829.811637	14.452787
18.889249	828.641702	14.457805
19.036720	838.265985	14.462823
18.575069	837.552291	14.467840
18.958168	827.362980	14.472858
18.680367	838.536666	14.477875
19.279369	855.683328	14.482893
19.332103	859.320184	14.487911
19.076572	861.881598	14.492928
19.353905	859.424490	14.497946
18.988245	851.279894	14.502963
19.495504	849.825222	14.507981
19.343829	854.888733	14.512999
19.423875	837.904989	14.518016
19.198976	832.023229	14.523034
18.871036	835.905538	14.528051
19.134103	842.091023	14.533069
19.312323	847.958370	14.538087
19.289999	863.989980	14.543104
19.566093	866.364483	14.548122
19.617330	865.296384	14.553139
19.492439	847.161141	14.558157
19.598154	851.976299	14.563175
19.186947	855.372971	14.568192
19.269760	852.529595	14.573210
19.204230	855.746218	14.578227
19.360360	857.890095	14.583245
19.700999	850.503356	14.588263
19.602758	849.212385	14.593280
19.743966	850.405556	14.598298
19.452423	843.297124	14.603315
19.881713	851.290208	14.608333
19.704348	848.925987	14.613351
19.684572	850.024305	14.618368
19.861873	843.616028	14.623386
19.728201	847.105184	14.628403
19.693513	857.925458	14.633421
19.537051	857.167402	14.638439
19.659268	854.854363	14.643456
20.077192	852.435325	14.648474
19.707692	852.609820	14.653491
19.720212	857.764529	14.658509
20.049831	857.877509	14.663527
19.625515	858.619102	14.668544
19.773421	846.844356	14.673562
19.794566	856.560900	14.678579
19.814154	858.486202	14.683597
19.775480	849.905697	14.688615
20.041960	847.983598	14.693632
19.878043	845.453185	14.698650
19.629601	849.231603	14.703667
19.373668	845.753022	14.708685
19.617180	839.511158	14.713703
19.254226	854.396620	14.718720
20.023911	862.724864	14.723738
19.956583	862.905959	14.728755
19.997487	872.240748	14.733773
20.202093	875.592036	14.738791
20.333135	878.086952	14.743808
20.241909	873.670715	14.748826
19.952884	878.632544	14.753843
19.787170	872.211394	14.758861
19.832104	879.901424	14.763879
19.771278	883.331909	14.768896
20.440390	875.960287	14.773914
20.149640	874.320600	14.778931
19.872676	866.708128	14.783949
20.250351	877.423186	14.788967
20.257132	874.594799	14.793984
20.068064	869.758306	14.799002
20.469553	881.176541	14.804019
20.385087	881.417108	14.809037
20.515162	880.286241	14.814055
20.457938	879.721011	14.819072
20.348159	874.771188	14.824090
20.617035	865.921890	14.829107
20.283791	869.287492	14.834125
20.283983	868.303078	14.839143
20.615488	880.256060	14.844160
20.832396	879.108518	14.849178
20.489637	877.338076	14.854195
20.693836	862.685996	14.859213
20.622479	866.648280	14.864231
20.344782	872.690759	14.869248
20.594960	879.638795	14.874266
20.899638	883.230117	14.879283
20.754288	877.566325	14.884301
20.915692	871.731700	14.889319
20.422302	871.613067	14.894336
20.719417	863.598797	14.899354
20.683339	879.765104	14.904371
21.075067	880.127183	14.909389
20.810984	872.626310	14.914407
20.831732	875.867372	14.919424
20.820637	867.516089	14.924442
20.704254	867.862608	14.929459
20.645790	885.600802	14.934477
21.012601	887.465733	14.939495
20.892765	889.371722	14.944512
21.161251	886.436317	14.949530
20.874259	883.480103	14.954547
20.643557	884.279913	14.959565
20.745834	888.275126	14.964583
20.533457	899.047353	14.969600
20.842036	895.692302	14.974618
21.203425	900.060576	14.979635
20.842697	893.594043	14.984653
20.717427	890.328633	14.989671
20.363383	894.663132	14.994688
20.997491	895.072679	14.999706
21.277390	907.163099	15.004723
21.016672	915.172127	15.009741
20.919418	917.251324	15.014759
21.130736	918.730223	15.019776
21.178631	917.075674	15.024794
21.353363	917.518877	15.029811
21.276224	922.993671	15.034829
21.393581	910.516754	15.039847
21.228751	917.295896	15.044864
21.075955	908.774156	15.049882
21.212012	910.649772	15.054899
21.074077	919.668455	15.059917
21.239819	916.064247	15.064935
20.996173	918.800540	15.069952
21.048216	918.473910	15.074970
21.164262	918.026865	15.079987
21.635928	927.032688	15.085005
21.817337	932.514566	15.090023
21.395990	925.814467	15.095040
21.709610	927.135431	15.100058
21.536558	933.464588	15.105075
21.599050	927.424444	15.110093
21.531645	911.934161	15.115111
21.669813	931.828711	15.120128
21.891182	925.609199	15.125146
21.652546	918.965861	15.130163
21.474368	918.438396	15.135181
21.788223	918.648503	15.140199
21.873448	926.379617	15.145216
21.540441	929.694701	15.150234
21.667839	927.503921	15.155251
21.755433	943.969759	15.160269
21.936774	936.970697	15.165287
21.656544	938.664983	15.170304
21.573481	936.740494	15.175322
22.001958	938.671567	15.180339
21.736912	937.371848	15.185357
21.918387	933.739940	15.190375
21.612766	932.967235	15.195392
21.984695	933.367112	15.200410
22.179428	942.782127	15.205427
22.360024	938.771666	15.210445
22.093990	936.667387	15.215463
21.733843	934.167514	15.220480
21.933356	933.167841	15.225498
21.857980	931.052812	15.230515
21.444912	930.678681	15.235533
21.836420	931.268009	15.240551
21.875199	936.513325	15.245568
21.854691	938.861436	15.250586
21.990138	949.655276	15.255603
22.081765	965.328415	15.260621
22.596179	963.048971	15.265639
22.233126	969.997848	15.270656
22.084318	957.347748	15.275674
22.478261	963.336177	15.280691
22.174603	966.763462	15.285709
22.310841	963.570929	15.290727
22.407292	969.381620	15.295744
22.216721	964.980828	15.300762
22.601436	961.197353	15.305779
22.362544	966.186115	15.310797
22.455757	957.301007	15.315815
22.358495	971.798067	15.320832
22.374466	971.546479	15.325850
22.662744	962.605752	15.330867
22.488925	967.470775	15.335885
22.479917	962.218065	15.340903
22.533442	977.534236	15.345920
22.480894	970.180264	15.350938
22.724465	966.182083	15.355955
22.533815	970.065135	15.360973
22.414850	971.510257	15.365991
22.600164	963.409210	15.371008
22.496432	971.598945	15.376026
22.619041	968.291771	15.381043
22.249333	971.227576	15.386061
22.675212	976.431568	15.391079
23.007420	984.420892	15.396096
23.153382	988.087440	15.401114
22.953658	971.838237	15.406131
22.634795	972.740137	15.411149
22.749322	983.458361	15.416167
22.887101	984.671010	15.421184
23.125887	987.461585	15.426202
23.255366	986.027853	15.431219
22.847430	988.000799	15.436237
23.176645	981.234311	15.441255
23.044424	977.752220	15.446272
22.831886	975.582803	15.451290
22.934699	987.704006	15.456307
22.984594	984.616429	15.461325
22.740287	991.022972	15.466343
22.823811	992.963579	15.471360
22.928521	997.867294	15.476378
23.047054	983.894317	15.481395
22.793617	988.244732	15.486413
23.061204	985.186376	15.491431
22.901835	982.753065	15.496448
23.141817	1006.888951	15.501466
23.385262	996.727599	15.506483
23.204337	1009.388446	15.511501
23.458015	1010.198049	15.516519
23.380450	1008.824953	15.521536
23.580634	1007.768368	15.526554
23.699775	1001.776183	15.531571
23.545766	998.029241	15.536589
23.513294	986.452898	15.541607
23.702344	990.343107	15.546624
23.495364	988.816596	15.551642
23.671571	982.679834	15.556659
23.559859	993.354395	15.561677
23.460105	988.668063	15.566695
23.849294	989.841568	15.571712
23.721583	991.240718	15.576730
23.584554	977.272822	15.581747
23.608255	988.295520	15.586765
23.610547	984.391704	15.591783
23.717765	982.144100	15.596800
23.469468	982.842513	15.601818
23.608572	977.983296	15.606835
23.579859	981.986302	15.611853
23.671775	995.797532	15.616871
23.928608	999.708747	15.621888
23.562663	1006.446653	15.626906
24.021655	1010.657748	15.631923
23.960332	1018.929263	15.636941
23.763296	1006.498073	15.641959
24.108863	1006.807384	15.646976
24.124390	1011.507241	15.651994
23.997706	1008.500801	15.657011
23.769955	1014.298870	15.662029
23.899807	1019.605768	15.667047
23.886264	1005.028499	15.672064
24.159921	1005.017652	15.677082
24.224638	1009.713005	15.682099
24.069099	1016.083646	15.687117
23.691344	1011.582600	15.692135
24.281532	1006.182936	15.697152
24.243438	1008.843058	15.702170
24.550970	1000.107593	15.707187
24.355316	999.668052	15.712205
24.263442	1002.103021	15.717223
24.100678	1011.374920	15.722240
24.026340	1004.617608	15.727258
24.527387	998.714282	15.732275
24.181500	1013.666645	15.737293
24.184037	1011.842428	15.742311
24.305858	1009.898654	15.747328
23.992274	1005.797866	15.752346
24.226886	999.402701	15.757363
23.712019	1017.202619	15.762381
23.730949	1023.650237	15.767399
24.229732	1027.621616	15.772416
24.085912	1030.443367	15.777434
24.548845	1035.114596	15.782451
24.405819	1032.924881	15.787469
24.466825	1033.922272	15.792487
24.561262	1042.907994	15.797504
24.617750	1058.927508	15.802522
25.026275	1054.581737	15.807539
24.854455	1046.892858	15.812557
24.699451	1043.209177	15.817575
25.034533	1033.696246	15.822592
24.979731	1028.283391	15.827610
25.019357	1023.922481	15.832627
24.921552	1024.105167	15.837645
24.862947	1032.073312	15.842663
24.938310	1030.020007	15.847680
24.452822	1029.262679	15.852698
24.683639	1022.972236	15.857715
24.916320	1033.700496	15.862733
24.928984	1040.278482	15.867751
25.364940	1048.437872	15.872768
25.080314	1039.239172	15.877786
24.913420	1035.383778	15.882803
24.826779	1032.913889	15.887821
25.370287	1043.464374	15.892839
25.149751	1027.130000	15.897856
24.898934	1037.356038	15.902874
25.158076	1035.154199	15.907891
24.815703	1045.429210	15.912909
25.001032	1048.209183	15.917927
25.115066	1052.647565	15.922944
25.280220	1062.414382	15.927962
25.490917	1052.955520	15.932979
25.592262	1051.119070	15.937997
25.074075	1054.592396	15.943015
25.516118	1046.514455	15.948032
25.209168	1050.955267	15.953050
25.582259	1049.470977	15.958067
25.634345	1043.501840	15.963085
25.528905	1049.116777	15.968103
25.705451	1043.585848	15.973120
25.586244	1044.655479	15.978138
25.421425	1047.130213	15.983155
25.602215	1042.949288	15.988173
25.296950	1046.799710	15.993191
25.555301	1044.683198	15.998208
25.299477	1049.097115	16.003226
25.574636	1048.009920	16.008243
25.260245	1052.148938	16.013261
25.400725	1039.409558	16.018279
25.413087	1044.665330	16.023296
25.543500	1053.127911	16.028314
25.795390	1066.930067	16.033331
25.943762	1067.490985	16.038349
26.225997	1067.437778	16.043367
26.014069	1051.423928	16.048384
25.601462	1045.618660	16.053402
26.007349	1057.244603	16.058419
25.928201	1063.313037	16.063437
25.821860	1067.520650	16.068455
26.102514	1068.278720	16.073472
26.041884	1073.451192	16.078490
26.220149	1071.328212	16.083507
26.207913	1075.524331	16.088525
26.123114	1073.432842	16.093543
26.003041	1054.848519	16.098560
25.818818	1059.557399	16.103578
25.868101	1073.309056	16.108595
26.260365	1077.322276	16.113613
25.887032	1075.518705	16.118631
26.232336	1078.927019	16.123648
26.367153	1077.514539	16.128666
26.091187	1073.663495	16.133683
26.560352	1070.371771	16.138701
26.200344	1079.554497	16.143719
26.155802	1070.731806	16.148736
25.751702	1071.435546	16.153754
26.096809	1072.458133	16.158771
26.491262	1078.938821	16.163789
26.057198	1087.173728	16.168807
26.528577	1083.730180	16.173824
26.459182	1095.527978	16.178842
26.506136	1088.486664	16.183859
26.671104	1092.213390	16.188877
26.553967	1092.777778	16.193895
26.895959	1085.277124	16.198912
26.961895	1092.026714	16.203930
26.978576	1087.363251	16.208947
26.890960	1072.298849	16.213965
26.586426	1067.840036	16.218983
26.819987	1066.333288	16.224000
26.561204	1058.910405	16.229018
26.500376	1078.381672	16.234035
26.776287	1078.361007	16.239053
26.646466	1087.182853	16.244071
27.148684	1084.940007	16.249088
27.076958	1093.913756	16.254106
26.782836	1085.098358	16.259123
27.031116	1074.683748	16.264141
26.981086	1086.244998	16.269159
27.019360	1085.443989	16.274176
27.299091	1079.281608	16.279194
27.111129	1088.260829	16.284211
27.401795	1091.024409	16.289229
26.989035	1098.564892	16.294247
27.282302	1085.432466	16.299264
27.084189	1093.753715	16.304282
26.858506	1092.416297	16.309299
27.140103	1086.370387	16.314317
26.872065	1082.486549	16.319335
27.145250	1076.798554	16.324352
27.208797	1078.060636	16.329370
26.797805	1091.262284	16.334387
27.358909	1095.716275	16.339405
27.149783	1092.915158	16.344423
27.121240	1085.241824	16.349440
26.857209	1093.017921	16.354458
27.203312	1107.878401	16.359475
27.465452	1109.737563	16.364493
28.061460	1107.262363	16.369511
28.232472	1113.661089	16.374528
27.901903	1102.026943	16.379546
27.323175	1088.844091	16.384563
27.571885	1092.541999	16.389581
27.805004	1105.394066	16.394599
27.950764	1100.489599	16.399616
27.610119	1097.248217	16.404634
27.461155	1102.866791	16.409651
27.933683	1102.692438	16.414669
27.957069	1113.276610	16.419687
27.785054	1108.964410	16.424704
28.008072	1109.513707	16.429722
27.911555	1103.267890	16.434739
27.841803	1101.663199	16.439757
27.594450	1110.942009	16.444775
27.903918	1104.118589	16.449792
27.778423	1104.930430	16.454810
27.690620	1119.965774	16.459827
27.967634	1115.176566	16.464845
27.645000	1110.345024	16.469863
27.619102	1111.709396	16.474880
27.612453	1111.145751	16.479898
27.427414	1125.612422	16.484915
28.125397	1133.475437	16.489933
28.127849	1136.952922	16.494951
28.336977	1132.133254	16.499968
28.439020	1140.025942	16.504986
28.229730	1134.769651	16.510003
28.529390	1139.223333	16.515021
28.344207	1143.711481	16.520039
28.296779	1135.312081	16.525056
28.372285	1135.540366	16.530074
28.436381	1134.422913	16.535091
28.808541	1132.033054	16.540109
28.470911	1138.583566	16.545127
28.915692	1133.600976	16.550144
29.000318	1128.422000	16.555162
28.810633	1125.229691	16.560179
28.727246	1114.109312	16.565197
28.347578	1117.053003	16.570215
28.468472	1107.560758	16.575232
28.451794	1106.951338	16.580250
28.662361	1130.479753	16.585267
28.977597	1123.030585	16.590285
28.970208	1131.218015	16.595303
28.877201	1114.103163	16.600320
28.782815	1107.658199	16.605338
28.555790	1108.145024	16.610355
28.999792	1116.909101	16.615373
28.956905	1122.523789	16.620391
28.424892	1121.767389	16.625408
28.587854	1129.723170	16.630426
28.879256	1127.809785	16.635443
29.348562	1124.035196	16.640461
29.164781	1126.787445	16.645479
29.320470	1125.551591	16.650496
28.974977	1126.438710	16.655514
28.784026	1130.485944	16.660531
28.869266	1122.154256	16.665549
29.164859	1122.767992	16.670567
28.857548	1117.867791	16.675584
29.069246	1121.596714	16.680602
28.979159	1123.021574	16.685619
29.530582	1123.324082	16.690637
29.207407	1117.643719	16.695655
28.799443	1123.069098	16.700672
29.247166	1129.311139	16.705690
29.029034	1143.448465	16.710707
29.342099	1146.972264	16.715725
29.471233	1150.300642	16.720743
29.329658	1146.700055	16.725760
29.550314	1151.547890	16.730778
29.468908	1154.643963	16.735795
29.537039	1148.877419	16.740813
29.555486	1148.167856	16.745831
29.262583	1156.794224	16.750848
29.302867	1145.985926	16.755866
29.464503	1158.735553	16.760883
29.690690	1162.572681	16.765901
29.764564	1169.273728	16.770919
29.592224	1173.737792	16.775936
29.924811	1170.085466	16.780954
29.723669	1177.829717	16.785971
29.936609	1170.522688	16.790989
30.071319	1173.178020	16.796007
30.052627	1175.314442	16.801024
30.176094	1167.093545	16.806042
29.785469	1175.905550	16.811059
29.996001	1168.065569	16.816077
30.272261	1178.692458	16.821095
30.064939	1176.768355	16.826112
30.079518	1173.528456	16.831130
29.786519	1178.282705	16.836147
29.795629	1172.506408	16.841165
30.296823	1175.322429	16.846183
30.182686	1162.609981	16.851200
30.225500	1169.625130	16.856218
30.214111	1174.906729	16.861235
30.359579	1169.948640	16.866253
30.477745	1172.328839	16.871271
30.211800	1174.516380	16.876288
30.255363	1164.420768	16.881306
30.127611	1169.316543	16.886323
30.219277	1170.590032	16.891341
30.504035	1165.717554	16.896359
30.640328	1167.132417	16.901376
30.369577	1163.533004	16.906394
30.460132	1172.159636	16.911411
30.686217	1163.799688	16.916429
30.575660	1161.466049	16.921447
30.454662	1165.256248	16.926464
30.864472	1178.465862	16.931482
30.918817	1185.946278	16.936499
30.832504	1170.196785	16.941517
30.704373	1166.224874	16.946535
30.658680	1170.820697	16.951552
31.228042	1167.977255	16.956570
30.763093	1175.513273	16.961587
31.099071	1172.567313	16.966605
31.152611	1173.957191	16.971623
30.745604	1177.249129	16.976640
31.021512	1157.782542	16.981658
31.083653	1172.340153	16.986675
30.920663	1168.578795	16.991693
31.160661	1176.879207	16.996711
31.247030	1178.481723	17.001728
31.159778	1182.146752	17.006746
31.122181	1188.729463	17.011763
31.664867	1173.582617	17.016781
31.279960	1154.698599	17.021799
31.085014	1154.539808	17.026816
31.190688	1168.219643	17.031834
31.284080	1181.866686	17.036851
31.199097	1184.202777	17.041869
31.479365	1187.457138	17.046887
31.429656	1183.188993	17.051904
31.368792	1175.997175	17.056922
31.730008	1186.737073	17.061939
31.817042	1178.455572	17.066957
31.539433	1174.027254	17.071975
31.331029	1181.106767	17.076992
31.748602	1182.645093	17.082010
31.569843	1187.965379	17.087027
31.378467	1180.238461	17.092045
31.355283	1179.595338	17.097063
31.352760	1189.388332	17.102080
31.679747	1180.473026	17.107098
31.354627	1175.468285	17.112115
31.401242	1181.084836	17.117133
31.999635	1193.110083	17.122151
32.148665	1202.415587	17.127168
32.095093	1184.275208	17.132186
31.532051	1182.895635	17.137203
31.710064	1188.984032	17.142221
32.179379	1197.182478	17.147239
32.160621	1206.507796	17.152256
32.300942	1201.152871	17.157274
32.251856	1203.978834	17.162291
32.290638	1204.089763	17.167309
32.371315	1196.973729	17.172327
32.152314	1194.022656	17.177344
31.738550	1193.071117	17.182362
32.271399	1198.242741	17.187379
32.149701	1196.800763	17.192397
32.446754	1197.284888	17.197415
32.208603	1204.403756	17.202432
32.276800	1191.877492	17.207450
32.119391	1196.629570	17.212467
32.103242	1203.089026	17.217485
32.626804	1195.613704	17.222503
32.333620	1199.875686	17.227520
32.477889	1201.380827	17.232538
32.244772	1210.193571	17.237555
31.913302	1198.423803	17.242573
32.680704	1207.352166	17.247591
32.375133	1216.498085	17.252608
32.603249	1219.265112	17.257626
32.866242	1219.432650	17.262643
32.794463	1213.536390	17.267661
32.760571	1223.189120	17.272679
32.803092	1225.871437	17.277696
32.923608	1217.568925	17.282714
32.741915	1220.626976	17.287731
32.845356	1219.740075	17.292749
33.272696	1215.224079	17.297767
33.144306	1214.546842	17.302784
33.002542	1219.874000	17.307802
33.528228	1225.690528	17.312819
33.079908	1220.061175	17.317837
33.066647	1205.988623	17.322855
32.818892	1216.914872	17.327872
33.306558	1219.212301	17.332890
33.105376	1232.163637	17.337907
33.310012	1222.008199	17.342925
33.411829	1223.728235	17.347943
33.140428	1221.634224	17.352960
33.049893	1220.102185	17.357978
33.254941	1223.238877	17.362995
32.763429	1222.510880	17.368013
33.049909	1219.547372	17.373031
33.371680	1233.048445	17.378048
33.710449	1237.574958	17.383066
33.914044	1242.122519	17.388083
33.889369	1239.756562	17.393101
33.795466	1223.998735	17.398119
33.448267	1217.163905	17.403136
33.563581	1223.968973	17.408154
33.692322	1234.076067	17.413171
33.905853	1245.056744	17.418189
33.795489	1238.910865	17.423207
33.666691	1244.822989	17.428224
33.870413	1239.492894	17.433242
33.697449	1245.408739	17.438259
33.799304	1250.688508	17.443277
33.694643	1243.187902	17.448295
33.745891	1242.962376	17.453312
33.815727	1248.117742	17.458330
33.711556	1236.429323	17.463347
33.536982	1240.647601	17.468365
33.987559	1252.752707	17.473383
34.396597	1259.395292	17.478400
34.269847	1259.715031	17.483418
34.244882	1255.790153	17.488435
33.904758	1256.616482	17.493453
34.619338	1265.764538	17.498471
34.334024	1271.177177	17.503488
34.430349	1268.053920	17.508506
34.517697	1270.483112	17.513523
34.075821	1264.792781	17.518541
34.406620	1254.466203	17.523559
34.325310	1258.862468	17.528576
34.216658	1259.343489	17.533594
34.518834	1259.211438	17.538611
34.475371	1265.122906	17.543629
34.692951	1264.369710	17.548647
34.408130	1265.802810	17.553664
34.586495	1256.863269	17.558682
34.636937	1261.671365	17.563699
34.419230	1267.247046	17.568717
34.757797	1252.507454	17.573735
34.589400	1258.485708	17.578752
34.931285	1255.930134	17.583770
34.732705	1255.759284	17.588787
35.053261	1261.857070	17.593805
34.948796	1270.858096	17.598823
34.781582	1270.407808	17.603840
34.390129	1278.932815	17.608858
34.660994	1281.753156	17.613875
35.129085	1283.857982	17.618893
35.184524	1272.469736	17.623911
34.937451	1282.026302	17.628928
35.022063	1276.667404	17.633946
35.008581	1273.943095	17.638963
34.757698	1276.576427	17.643981
35.308845	1282.597293	17.648999
35.764760	1295.582066	17.654016
35.345021	1291.166380	17.659034
35.248774	1272.398240	17.664051
35.443033	1294.550326	17.669069
35.631029	1291.160328	17.674087
35.626925	1278.449601	17.679104
35.517693	1278.378449	17.684122
35.639975	1278.520558	17.689139
35.688966	1289.867708	17.694157
35.709014	1282.104672	17.699175
35.748329	1280.722825	17.704192
35.699496	1278.764567	17.709210
35.710807	1285.910899	17.714227
36.016277	1300.156174	17.719245
36.194332	1288.632062	17.724263
35.961971	1286.727624	17.729280
35.885552	1286.045449	17.734298
36.052556	1271.600796	17.739315
35.967996	1275.224400	17.744333
35.654259	1265.190672	17.749351
35.936553	1284.081723	17.754368
35.985367	1288.296789	17.759386
36.146291	1304.189810	17.764403
36.230580	1298.193484	17.769421
36.255523	1287.914508	17.774439
36.327228	1300.883366	17.779456
36.560960	1299.057837	17.784474
36.270475	1295.985333	17.789491
36.339682	1300.263498	17.794509
36.430089	1293.581412	17.799527
36.341180	1300.342566	17.804544
36.147345	1297.523257	17.809562
36.494879	1285.600375	17.814579
36.383789	1293.520004	17.819597
36.443420	1295.776790	17.824615
36.210542	1290.202233	17.829632
35.959611	1294.211505	17.834650
36.396205	1293.657738	17.839667
36.380220	1307.489165	17.844685
36.812386	1305.954632	17.849703
36.858210	1320.211947	17.854720
36.619262	1320.145211	17.859738
36.971542	1317.338701	17.864755
36.785020	1326.412491	17.869773
37.153027	1319.314788	17.874791
36.861196	1331.122128	17.879808
37.073902	1326.222955	17.884826
37.222594	1308.196125	17.889843
36.807497	1325.075099	17.894861
37.173011	1317.614867	17.899879
36.962785	1315.710135	17.904896
37.412842	1315.823303	17.909914
37.140597	1316.048930	17.914931
37.090116	1313.964693	17.919949
37.496662	1308.066512	17.924967
37.291618	1312.478898	17.929984
36.995666	1315.419055	17.935002
37.308868	1313.347621	17.940019
37.144294	1314.670484	17.945037
37.243299	1312.607154	17.950055
36.966290	1314.020106	17.955072
37.244805	1320.367455	17.960090
37.330400	1310.905845	17.965107
36.899403	1324.508411	17.970125
37.405727	1328.008469	17.975143
37.641347	1338.875311	17.980160
37.395095	1344.004179	17.985178
37.613320	1336.194485	17.990195
37.675684	1335.124626	17.995213
37.522315	1336.707678	18.000231
38.192821	1335.435836	18.005248
37.521284	1339.277075	18.010266
38.060046	1337.145273	18.015283
37.974372	1344.278326	18.020301
37.792826	1339.762426	18.025319
37.673484	1343.012761	18.030336
37.964595	1353.258745	18.035354
38.126088	1353.047611	18.040371
38.244649	1362.133880	18.045389
38.239731	1364.309205	18.050407
38.579997	1363.079311	18.055424
38.170752	1360.978342	18.060442
38.372122	1354.799666	18.065459
38.384721	1354.450767	18.070477
38.588796	1351.844052	18.075495
38.504712	1347.669583	18.080512
38.064604	1345.485059	18.085530
38.438242	1350.441674	18.090547
38.485257	1361.249533	18.095565
38.482136	1362.398938	18.100583
38.657466	1363.599455	18.105600
38.842547	1367.544014	18.110618
39.150045	1355.927121	18.115635
38.577813	1367.967492	18.120653
38.876362	1359.062837	18.125671
38.545967	1359.022963	18.130688
38.163882	1358.634529	18.135706
38.678910	1363.338760	18.140723
38.395650	1359.712852	18.145741
38.478062	1360.037896	18.150759
38.462007	1380.853211	18.155776
38.803590	1376.561967	18.160794
38.932339	1385.804452	18.165811
39.157588	1386.621656	18.170829
38.983835	1390.044574	18.175847
39.206186	1386.175836	18.180864
39.107842	1381.006340	18.185882
39.314024	1370.339335	18.190899
38.968141	1386.301870	18.195917
38.947796	1381.476837	18.200935
39.099084	1380.503584	18.205952
39.370609	1396.133314	18.210970
39.294495	1398.903555	18.215987
39.252783	1401.094081	18.221005
39.349259	1398.958551	18.226023
39.742580	1400.699490	18.231040
39.804396	1410.564639	18.236058
40.027845	1406.001444	18.241075
39.978598	1402.301223	18.246093
39.772255	1382.786399	18.251111
39.515368	1385.225021	18.256128
39.575560	1395.346035	18.261146
39.815862	1396.855177	18.266163
40.013271	1402.236878	18.271181
39.741727	1404.261216	18.276199
40.113502	1390.280050	18.281216
40.213360	1392.502183	18.286234
39.954090	1393.931314	18.291251
40.037487	1392.716164	18.296269
40.134682	1397.911495	18.301287
40.063169	1394.688116	18.306304
39.960707	1393.902693	18.311322
40.303057	1387.869313	18.316339
40.321589	1402.389720	18.321357
40.084858	1389.538407	18.326375
40.043745	1391.388010	18.331392
39.985648	1399.829613	18.336410
40.340126	1393.279944	18.341427
40.216026	1390.856864	18.346445
39.881327	1403.055935	18.351463
40.421072	1412.231288	18.356480
40.259994	1422.169017	18.361498
40.661624	1418.417527	18.366515
40.670618	1414.370562	18.371533
40.190752	1427.529532	18.376551
40.829648	1418.275210	18.381568
40.550950	1423.910928	18.386586
40.755059	1425.946419	18.391603
40.718560	1423.273008	18.396621
40.601750	1422.524532	18.401639
40.948981	1424.910126	18.406656
40.997926	1432.072747	18.411674
41.308224	1436.464888	18.416691
41.295217	1421.880883	18.421709
40.877475	1425.212407	18.426727
41.209280	1426.584227	18.431744
40.924745	1445.390131	18.436762
41.046290	1429.475500	18.441779
41.251539	1440.997234	18.446797
41.527242	1437.154893	18.451815
41.516352	1437.159947	18.456832
41.298864	1442.924998	18.461850
41.771409	1439.361280	18.466867
41.671364	1441.440972	18.471885
41.486443	1451.795844	18.476903
41.553469	1441.617525	18.481920
41.622984	1441.862527	18.486938
41.663982	1435.191236	18.491955
41.813492	1445.049062	18.496973
41.623657	1448.335639	18.501991
41.814292	1445.238693	18.507008
41.722005	1446.988971	18.512026
41.547291	1440.136668	18.517043
42.051180	1441.043036	18.522061
41.953766	1441.711662	18.527079
41.914051	1435.630455	18.532096
41.707445	1434.602467	18.537114
42.143604	1435.585652	18.542131
42.060974	1431.707584	18.547149
41.694513	1437.915553	18.552167
41.916585	1427.126119	18.557184
41.828830	1436.064666	18.562202
42.281148	1446.222488	18.567219
42.632515	1456.812603	18.572237
42.263015	1454.550799	18.577255
42.210639	1447.698380	18.582272
42.228205	1447.683224	18.587290
42.514807	1459.047135	18.592307
42.834846	1457.435372	18.597325
42.605935	1453.961931	18.602343
42.609774	1456.375747	18.607360
42.511895	1457.117031	18.612378
42.954631	1458.209648	18.617395
42.743529	1443.927868	18.622413
42.554502	1451.799741	18.627431
42.722276	1454.431032	18.632448
42.563376	1454.020471	18.637466
42.470168	1453.334591	18.642483
42.666187	1451.877839	18.647501
42.372856	1453.195512	18.652519
42.634198	1450.488348	18.657536
42.871771	1465.164052	18.662554
43.015572	1478.954955	18.667571
43.212278	1476.125305	18.672589
43.118640	1487.633644	18.677607
43.273216	1475.598666	18.682624
43.134653	1480.070171	18.687642
43.164652	1483.846395	18.692659
43.461435	1480.840215	18.697677
43.107815	1478.897831	18.702695
43.615894	1475.495833	18.707712
43.571060	1486.068757	18.712730
43.315848	1480.229371	18.717747
43.426039	1471.413949	18.722765
43.320341	1482.659072	18.727783
43.361644	1481.153822	18.732800
43.118639	1488.970998	18.737818
43.729601	1494.537651	18.742835
44.064197	1491.405660	18.747853
44.208682	1484.582536	18.752871
43.936183	1471.821940	18.757888
44.071544	1481.107627	18.762906
44.053831	1470.162994	18.767923
44.262541	1468.350811	18.772941
43.646219	1475.291979	18.777959
43.953417	1464.716488	18.782976
44.038131	1483.114644	18.787994
43.871135	1486.489191	18.793011
44.479912	1491.084185	18.798029
44.309567	1498.161054	18.803047
44.094537	1499.217228	18.808064
44.073411	1501.515016	18.813082
44.570969	1497.770665	18.818099
44.782933	1495.440415	18.823117
44.642442	1494.569389	18.828135
44.678263	1491.622773	18.833152
44.047083	1496.622266	18.838170
44.621779	1495.163357	18.843187
44.525437	1489.406531	18.848205
44.409334	1495.581852	18.853223
44.328535	1496.595036	18.858240
44.591872	1496.746745	18.863258
44.691734	1490.624851	18.868275
44.728705	1497.997649	18.873293
44.779761	1509.281500	18.878311
44.876769	1512.289896	18.883328
45.129483	1507.381288	18.888346
45.024612	1517.827877	18.893363
45.232539	1512.449710	18.898381
45.217050	1521.225567	18.903399
45.156949	1520.837491	18.908416
44.974952	1519.562667	18.913434
45.033334	1509.565539	18.918451
45.247464	1509.106364	18.923469
45.315912	1510.203610	18.928487
45.493449	1513.634974	18.933504
45.472197	1513.616395	18.938522
45.561040	1517.127841	18.943539
45.554696	1510.820503	18.948557
45.223859	1518.272667	18.953575
45.198413	1514.663391	18.958592
45.273909	1514.926398	18.963610
45.219303	1514.029376	18.968627
45.622818	1519.145492	18.973645
45.276927	1537.241513	18.978663
45.536919	1526.976297	18.983680
45.703697	1529.039702	18.988698
45.768686	1526.359942	18.993715
45.940513	1520.892717	18.998733
46.115762	1533.820377	19.003751
45.787933	1530.548516	19.008768
45.956060	1536.117857	19.013786
45.887526	1547.035338	19.018803
46.450166	1551.306167	19.023821
46.394478	1562.411008	19.028839
46.313886	1555.951110	19.033856
46.444327	1552.194478	19.038874
46.445840	1551.774717	19.043891
46.699464	1551.681783	19.048909
46.640328	1554.496743	19.053927
46.372876	1547.892369	19.058944
46.574277	1549.366554	19.063962
46.308633	1554.971879	19.068979
46.596523	1547.302728	19.073997
46.407931	1557.718193	19.079015
46.287458	1553.382081	19.084032
46.397714	1554.491755	19.089050
46.596796	1555.900029	19.094067
46.385741	1557.984395	19.099085
46.636626	1576.416736	19.104103
46.548086	1573.019247	19.109120
46.793971	1571.936580	19.114138
46.807239	1571.104727	19.119155
47.025956	1580.298592	19.124173
47.202917	1573.334677	19.129191
47.279388	1581.487166	19.134208
47.266608	1571.368538	19.139226
47.053072	1569.858775	19.144243
47.401304	1581.172143	19.149261
47.631516	1596.893690	19.154279
47.610088	1600.434945	19.159296
48.302521	1597.297715	19.164314
47.577814	1581.647253	19.169331
47.542800	1578.995679	19.174349
47.601271	1574.382388	19.179367
47.324573	1570.010634	19.184384
47.570726	1576.091710	19.189402
47.321898	1583.995043	19.194419
47.612068	1588.664915	19.199437
47.536039	1598.958735	19.204455
47.770115	1601.604972	19.209472
48.004227	1597.333564	19.214490
47.764279	1605.229212	19.219507
47.709909	1600.863861	19.224525
48.105587	1610.115397	19.229543
48.244016	1629.739281	19.234560
48.403207	1621.957590	19.239578
47.815092	1617.801571	19.244595
48.135214	1618.607170	19.249613
48.135129	1622.025184	19.254631
48.038194	1626.862636	19.259648
48.499405	1613.059879	19.264666
48.440126	1620.438246	19.269683
48.407538	1615.072248	19.274701
48.424914	1622.280887	19.279719
48.382498	1629.940660	19.284736
48.491215	1617.234216	19.289754
48.493379	1614.870343	19.294771
48.741648	1630.197780	19.299789
49.140539	1640.512357	19.304807
49.227791	1633.521360	19.309824
49.195482	1625.457053	19.314842
48.669914	1627.527278	19.319859
48.926799	1617.496027	19.324877
48.592874	1617.851183	19.329895
48.865440	1628.646178	19.334912
48.839773	1638.099032	19.339930
49.043912	1645.224952	19.344947
49.216816	1642.313774	19.349965
49.193042	1642.847864	19.354983
49.429785	1644.868831	19.360000
49.554899	1640.649098	19.365018
49.689345	1644.286015	19.370035
49.662882	1636.081935	19.375053
49.643889	1637.104439	19.380071
49.454377	1636.521910	19.385088
49.660573	1632.264308	19.390106
49.296405	1638.774952	19.395123
49.407883	1631.884327	19.400141
49.767593	1645.275662	19.405159
49.975780	1662.701708	19.410176
50.069820	1659.458816	19.415194
50.098148	1657.169760	19.420211
50.190776	1651.405551	19.425229
50.349574	1648.689076	19.430247
49.721798	1642.781409	19.435264
50.020117	1640.784840	19.440282
49.901436	1656.601787	19.445299
50.263791	1654.866651	19.450317
49.929525	1655.900372	19.455335
49.997432	1657.013491	19.460352
50.492223	1656.267613	19.465370
49.987641	1660.846645	19.470387
50.754213	1650.186899	19.475405
50.604103	1649.721314	19.480423
50.566751	1655.379490	19.485440
50.478621	1658.217916	19.490458
50.312020	1666.566083	19.495475
50.641975	1674.448770	19.500493
50.922456	1673.483790	19.505511
50.854529	1682.327852	19.510528
51.162880	1676.526892	19.515546
50.640591	1682.724492	19.520563
50.558552	1684.501601	19.525581
50.959218	1679.724549	19.530599
51.185428	1680.143978	19.535616
51.458681	1673.101914	19.540634
51.107208	1683.091523	19.545651
51.058848	1676.544510	19.550669
50.934175	1674.184597	19.555687
51.098996	1676.750108	19.560704
51.236962	1682.759701	19.565722
51.085621	1702.081635	19.570739
51.125987	1700.314575	19.575757
51.213325	1694.649008	19.580775
51.220876	1699.050480	19.585792
51.508220	1699.331000	19.590810
51.432191	1697.215981	19.595827
51.504033	1709.067935	19.600845
51.688433	1720.173364	19.605863
51.735201	1718.648308	19.610880
52.202522	1722.801472	19.615898
52.085196	1728.418473	19.620915
52.176935	1722.080010	19.625933
52.043331	1721.968468	19.630951
52.055645	1724.756550	19.635968
52.265647	1722.088898	19.640986
52.285123	1721.035161	19.646003
52.282704	1723.345843	19.651021
52.321115	1716.292989	19.656039
52.053228	1721.021380	19.661056
52.307070	1712.379137	19.666074
52.099096	1712.995558	19.671091
52.216650	1714.700568	19.676109
52.700858	1723.796364	19.681127
52.283481	1718.221996	19.686144
51.954941	1715.066979	19.691162
52.631199	1736.825826	19.696179
52.908807	1739.471618	19.701197
52.544344	1732.017568	19.706215
52.375440	1747.962338	19.711232
52.472277	1744.690593	19.716250
52.482088	1742.218212	19.721267
52.840698	1747.341385	19.726285
53.236066	1758.944180	19.731303
52.974573	1773.341225	19.736320
53.233838	1762.410095	19.741338
53.553510	1768.839562	19.746355
53.501704	1762.551837	19.751373
53.600988	1763.155135	19.756391
53.409965	1767.082599	19.761408
53.676119	1757.135037	19.766426
53.411998	1763.311404	19.771443
53.372021	1763.737564	19.776461
53.656700	1760.158852	19.781479
53.488969	1763.489382	19.786496
53.795882	1762.283590	19.791514
53.569833	1762.899671	19.796531
53.744129	1760.635213	19.801549
53.779019	1755.703647	19.806567
53.443194	1753.427093	19.811584
53.618568	1761.198184	19.816602
54.310018	1776.753399	19.821619
54.523726	1781.435227	19.826637
54.341013	1770.667583	19.831655
54.483238	1761.749197	19.836672
54.076317	1753.007836	19.841690
54.323527	1761.054927	19.846707
54.290543	1769.527509	19.851725
54.593765	1759.236494	19.856743
54.459713	1777.555403	19.861760
54.570727	1772.880230	19.866778
54.534652	1768.710810	19.871795
54.753650	1770.302198	19.876813
54.972731	1771.940911	19.881831
54.568625	1783.447285	19.886848
54.564452	1763.171557	19.891866
54.750559	1772.578886	19.896883
54.668809	1766.930155	19.901901
54.759508	1772.085580	19.906919
54.617887	1780.089075	19.911936
54.815238	1773.639473	19.916954
55.035017	1784.789929	19.921971
55.159650	1803.355773	19.926989
55.354880	1799.011474	19.932007
55.433536	1801.943879	19.937024
55.804695	1798.449526	19.942042
55.374156	1802.714100	19.947059
55.231077	1806.148101	19.952077
55.725678	1800.460118	19.957095
55.600840	1805.270404	19.962112
55.546633	1788.597000	19.967130
55.807968	1802.407724	19.972147
55.354532	1800.278867	19.977165
55.697546	1800.241444	19.982183
55.528420	1800.583568	19.987200
55.626364	1792.748221	19.992218
55.588678	1793.082504	19.997235
55.329379	1804.582125	20.002253
55.949577	1809.506793	20.007271
55.894890	1823.524532	20.012288
56.237920	1819.608509	20.017306
56.172528	1831.721759	20.022323
56.402709	1828.489199	20.027341
56.539991	1824.324334	20.032359
56.220842	1826.545485	20.037376
56.318980	1825.378505	20.042394
56.111073	1823.072559	20.047411
56.229786	1829.738470	20.052429
56.104110	1817.185146	20.057447
56.282392	1843.742878	20.062464
56.434720	1849.914397	20.067482
56.575819	1850.309211	20.072499
56.730922	1851.998920	20.077517
57.040174	1841.419731	20.082535
56.749293	1845.280707	20.087552
57.114616	1842.768740	20.092570
57.115245	1835.989972	20.097587
57.207538	1828.546820	20.102605
57.442568	1825.884723	20.107623
57.627046	1828.074800	20.112640
57.444832	1835.554449	20.117658
57.796367	1830.459949	20.122675
57.337474	1832.819626	20.127693
57.802468	1828.177691	20.132711
57.421961	1835.467300	20.137728
57.555847	1826.547025	20.142746
57.583295	1822.168880	20.147763
57.586059	1820.104697	20.152781
57.732326	1827.918219	20.157799
57.480272	1830.482384	20.162816
57.488374	1826.082004	20.167834
57.599340	1830.063452	20.172851
57.933003	1839.539364	20.177869
58.175649	1838.116348	20.182887
58.161149	1833.574314	20.187904
58.347309	1846.734039	20.192922
58.287899	1840.037203	20.197939
58.136368	1838.337877	20.202957
58.385820	1837.207300	20.207975
57.768876	1835.678270	20.212992
57.558751	1854.488799	20.218010
57.957667	1845.539873	20.223027
58.267544	1859.380954	20.228045
58.881231	1866.010840	20.233063
58.603616	1872.852086	20.238080
58.479732	1868.690003	20.243098
58.659443	1863.947304	20.248115
58.645129	1876.999404	20.253133
58.652037	1866.003356	20.258151
58.548985	1872.798488	20.263168
58.808641	1896.392857	20.268186
58.959464	1898.944800	20.273203
59.111647	1901.345048	20.278221
59.280038	1896.998592	20.283239
59.024940	1895.167058	20.288256
58.818840	1895.442355	20.293274
59.369086	1892.276719	20.298291
59.366255	1893.700678	20.303309
59.178690	1886.424155	20.308327
59.463100	1899.227783	20.313344
59.576808	1903.502321	20.318362
59.985268	1908.627247	20.323379
59.733267	1903.380533	20.328397
59.985580	1898.456103	20.333415
59.786947	1896.202353	20.338432
59.867440	1900.598830	20.343450
60.090324	1911.540591	20.348467
60.208695	1916.328820	20.353485
59.979018	1908.143630	20.358503
59.855215	1902.747564	20.363520
59.765096	1912.336835	20.368538
60.046489	1915.133548	20.373555
59.936306	1921.642620	20.378573
59.607540	1915.278038	20.383591
60.202716	1921.077665	20.388608
60.148986	1933.820352	20.393626
60.497392	1933.283454	20.398643
60.294508	1943.168019	20.403661
60.687365	1938.218539	20.408679
60.668067	1933.434221	20.413696
60.515592	1947.309486	20.418714
60.623654	1931.645825	20.423731
60.835805	1944.804731	20.428749
61.182107	1957.677663	20.433767
61.095757	1947.106355	20.438784
61.213299	1960.396772	20.443802
61.159350	1946.626628	20.448819
61.071026	1954.549317	20.453837
61.318342	1956.414034	20.458855
61.337670	1954.161056	20.463872
61.452008	1961.881775	20.468890
61.486678	1952.901141	20.473907
61.499779	1967.593273	20.478925
61.437383	1956.172444	20.483943
61.563520	1953.129636	20.488960
61.556492	1957.385114	20.493978
61.606624	1948.711355	20.498995
61.711994	1958.112418	20.504013
62.031019	1951.959400	20.509031
62.058032	1950.592040	20.514048
61.530337	1952.782557	20.519066
62.083101	1959.355689	20.524083
62.162694	1976.675826	20.529101
62.342688	1978.005052	20.534119
62.333584	1979.994905	20.539136
62.165465	1985.155973	20.544154
62.841415	1966.105923	20.549171
62.572147	1972.712369	20.554189
62.383028	1976.024177	20.559207
62.727544	1969.157102	20.564224
62.507062	1977.870423	20.569242
62.606547	1971.448611	20.574259
62.409267	1970.333930	20.579277
62.621776	1961.391878	20.584295
62.889125	1970.253312	20.589312
62.387095	1964.316490	20.594330
63.134865	1969.540090	20.599347
63.048632	1994.239363	20.604365
62.956743	1996.242107	20.609383
62.888220	1992.153430	20.614400
63.280631	1998.161384	20.619418
63.110268	1985.135199	20.624435
63.094160	1993.860890	20.629453
63.009063	1998.109597	20.634471
62.823978	1998.056562	20.639488
63.141962	2002.545481	20.644506
63.493504	2010.721614	20.649523
63.621152	2018.348763	20.654541
63.596155	2009.775039	20.659559
63.849127	2011.670440	20.664576
63.868139	2016.038647	20.669594
63.876706	2018.196173	20.674611
63.771697	2013.923815	20.679629
63.914984	2003.108429	20.684647
64.151344	2016.197344	20.689664
63.847114	2024.062157	20.694682
64.198817	2032.560180	20.699699
64.482751	2040.983548	20.704717
64.704049	2031.364723	20.709735
64.654075	2021.620874	20.714752
64.613932	2017.455186	20.719770
64.811544	2006.653431	20.724787
64.313312	2002.735801	20.729805
64.358711	2025.988144	20.734823
64.512915	2024.140209	20.739840
64.491510	2031.910496	20.744858
64.789007	2026.470890	20.749875
64.783802	2030.931237	20.754893
64.740122	2037.048129	20.759911
64.957362	2029.983088	20.764928
64.670877	2046.419821	20.769946
65.229240	2047.374548	20.774963
65.490582	2059.913628	20.779981
65.298757	2052.161154	20.784999
65.388097	2051.702460	20.790016
65.419189	2054.370902	20.795034
65.456484	2045.916854	20.800051
65.590803	2038.921527	20.805069
65.266928	2048.638787	20.810087
65.455522	2049.455418	20.815104
65.573418	2062.045237	20.820122
65.456757	2066.958466	20.825139
65.491125	2078.261054	20.830157
65.756534	2074.754710	20.835175
66.401647	2070.128852	20.840192
65.744241	2066.264394	20.845210
66.308626	2063.951787	20.850227
66.286428	2075.231621	20.855245
66.178856	2070.735577	20.860263
66.667139	2091.002961	20.865280
66.532783	2096.010475	20.870298
66.583428	2082.031429	20.875315
66.399108	2084.294738	20.880333
66.835757	2094.887735	20.885351
66.778043	2089.285655	20.890368
66.760410	2098.494493	20.895386
67.151763	2095.511359	20.900403
67.132278	2105.001369	20.905421
67.046444	2103.231826	20.910439
67.250924	2087.256359	20.915456
67.196164	2091.572951	20.920474
67.346836	2089.949631	20.925491
66.799752	2096.024995	20.930509
66.856390	2089.098550	20.935527
67.339486	2095.357517	20.940544
66.961782	2093.368319	20.945562
67.446261	2088.732751	20.950579
67.953957	2099.055902	20.955597
67.487638	2101.672401	20.960615
67.676578	2106.724261	20.965632
67.728399	2119.699966	20.970650
67.692164	2116.272138	20.975667
68.036483	2111.958202	20.980685
67.886666	2117.940161	20.985703
68.275664	2108.333056	20.990720
67.983618	2107.431945	20.995738
67.902259	2106.551682	21.000755
68.035267	2104.962670	21.005773
67.768416	2112.067431	21.010791
68.241113	2105.546437	21.015808
68.151163	2114.574030	21.020826
68.088956	2131.648139	21.025843
67.856384	2138.217373	21.030861
68.457953	2137.057203	21.035879
68.335247	2129.243438	21.040896
68.419481	2142.207801	21.045914
68.795907	2150.900857	21.050931
69.014054	2155.080295	21.055949
69.098956	2162.859335	21.060967
69.113021	2155.731199	21.065984
69.360183	2158.567996	21.071002
69.328052	2152.920885	21.076019
69.751664	2152.810950	21.081037
69.424889	2158.047265	21.086055
69.374076	2146.340475	21.091072
69.157231	2154.822930	21.096090
69.652332	2157.617968	21.101107
69.746679	2154.207673	21.106125
69.506995	2151.467953	21.111143
69.861630	2143.213772	21.116160
69.460508	2153.397573	21.121178
69.663738	2154.470719	21.126195
69.691384	2147.132178	21.131213
69.769200	2168.441904	21.136231
69.834466	2164.370228	21.141248
69.896053	2163.590789	21.146266
70.333833	2168.300951	21.151283
70.451998	2160.465450	21.156301
70.264142	2163.587739	21.161319
70.316034	2163.374725	21.166336
69.701000	2168.646456	21.171354
69.644651	2181.702167	21.176371
70.007817	2177.562015	21.181389
70.105877	2188.330867	21.186407
70.740445	2194.342213	21.191424
71.035384	2210.723287	21.196442
71.227771	2215.515852	21.201459
71.037034	2209.426334	21.206477
70.991268	2208.161809	21.211495
71.164052	2207.668027	21.216512
71.277780	2206.782633	21.221530
71.314601	2211.684629	21.226547
71.364334	2214.934045	21.231565
70.961921	2219.566741	21.236583
71.250156	2207.213801	21.241600
71.219572	2216.655102	21.246618
71.782974	2228.746464	21.251635
71.883932	2230.510915	21.256653
71.797183	2242.119657	21.261671
71.893872	2236.165270	21.266688
71.813189	2235.641520	21.271706
72.059822	2229.701661	21.276723
72.094417	2231.356517	21.281741
71.900404	2228.180463	21.286759
72.398435	2222.135190	21.291776
72.491412	2227.883714	21.296794
72.430178	2228.035469	21.301811
72.240110	2223.599570	21.306829
71.897659	2224.883918	21.311847
72.538853	2240.756650	21.316864
72.505945	2240.727261	21.321882
72.426839	2243.251933	21.326899
72.782671	2245.876154	21.331917
72.659405	2251.797217	21.336935
73.009163	2249.243434	21.341952
73.110840	2248.290483	21.346970
72.817016	2247.721018	21.351987
73.377947	2241.659633	21.357005
72.939977	2251.726144	21.362023
73.244785	2249.444461	21.367040
73.341019	2242.477076	21.372058
73.184319	2253.872643	21.377075
73.521657	2257.336078	21.382093
73.248885	2269.210499	21.387111
73.702881	2269.528202	21.392128
73.957048	2267.349081	21.397146
73.481254	2272.201510	21.402163
73.811379	2271.055190	21.407181
73.445462	2278.408982	21.412199
73.744801	2264.605680	21.417216
73.947624	2273.559367	21.422234
73.988168	2284.280424	21.427251
74.685833	2292.898286	21.432269
74.389680	2292.704744	21.437287
74.527234	2292.942321	21.442304
74.486680	2303.499281	21.447322
74.658812	2303.889274	21.452339
74.518420	2286.944785	21.457357
74.490958	2299.125034	21.462375
74.412322	2287.233124	21.467392
74.548625	2292.539399	21.472410
74.510126	2287.647516	21.477427
75.031788	2303.447391	21.482445
74.654317	2306.523483	21.487463
75.059736	2317.153035	21.492480
75.358638	2318.773060	21.497498
75.001125	2314.448420	21.502515
75.346160	2313.861542	21.507533
75.068987	2312.071273	21.512551
75.473997	2304.052186	21.517568
75.727521	2321.774790	21.522586
75.496481	2328.258643	21.527603
75.779667	2326.873461	21.532621
75.774270	2334.284761	21.537639
75.865256	2330.328970	21.542656
76.102713	2338.257913	21.547674
75.864725	2346.229325	21.552691
75.760324	2334.739050	21.557709
75.852990	2339.616606	21.562727
76.214277	2323.856369	21.567744
76.142761	2338.363152	21.572762
76.080059	2350.646758	21.577779
76.290798	2354.256163	21.582797
76.230464	2357.096683	21.587815
76.506205	2355.415995	21.592832
76.625078	2351.518978	21.597850
76.489919	2354.481608	21.602867
77.084750	2373.909011	21.607885
77.128541	2376.853250	21.612903
77.238782	2386.585159	21.617920
77.513118	2378.731560	21.622938
77.153818	2374.549204	21.627955
77.470943	2372.461260	21.632973
77.520957	2379.857639	21.637991
77.128346	2384.968562	21.643008
77.367943	2371.935074	21.648026
77.307536	2376.845941	21.653043
77.856805	2376.807965	21.658061
77.512578	2378.843727	21.663079
77.267879	2374.350021	21.668096
77.574452	2362.988256	21.673114
77.490717	2374.552431	21.678131
77.510541	2376.872359	21.683149
77.747386	2396.727931	21.688167
77.884487	2393.383523	21.693184
77.743856	2392.528254	21.698202
77.848343	2399.862508	21.703219
77.923648	2418.929008	21.708237
78.242253	2420.299806	21.713255
78.304535	2430.329558	21.718272
78.259669	2422.768651	21.723290
78.359297	2429.339921	21.728307
78.779083	2431.572336	21.733325
78.670493	2440.435727	21.738343
78.812130	2437.220001	21.743360
79.299783	2440.199292	21.748378
78.446269	2446.407694	21.753395
79.109148	2441.630645	21.758413
79.248589	2438.528876	21.763431
79.258275	2438.019454	21.768448
79.654738	2444.118453	21.773466
79.149386	2454.795210	21.778483
79.813386	2459.116755	21.783501
79.376571	2468.769770	21.788519
79.710805	2469.478533	21.793536
80.213140	2463.208433	21.798554
79.632616	2458.864827	21.803571
79.869987	2458.847008	21.808589
80.251789	2467.103852	21.813607
79.787012	2470.641718	21.818624
79.885320	2468.944461	21.823642
80.135627	2478.566244	21.828659
80.471737	2479.375708	21.833677
80.481078	2486.832116	21.838695
80.338752	2497.278795	21.843712
80.683095	2488.896662	21.848730
80.813723	2487.592029	21.853747
80.815526	2483.811047	21.858765
81.036581	2483.486479	21.863783
81.097289	2492.386658	21.868800
80.774974	2483.316163	21.873818
80.662281	2488.191017	21.878835
81.045808	2488.292463	21.883853
81.001446	2493.626926	21.888871
80.783265	2504.328433	21.893888
81.212897	2508.913714	21.898906
81.318778	2508.758567	21.903923
81.505875	2500.407223	21.908941
81.379280	2523.030539	21.913959
81.494037	2527.371339	21.918976
81.676285	2524.868846	21.923994
81.827301	2537.125617	21.929011
81.855460	2533.899137	21.934029
81.952906	2531.788569	21.939047
82.074330	2530.497991	21.944064
82.267399	2521.542907	21.949082
82.125034	2540.621334	21.954099
82.405311	2540.581055	21.959117
82.700479	2544.773842	21.964135
82.541543	2553.780837	21.969152
82.612350	2546.978250	21.974170
82.658515	2531.484660	21.979187
83.364683	2534.284768	21.984205
83.108666	2534.012385	21.989223
82.710077	2541.002117	21.994240
83.166338	2541.540395	21.999258
83.154604	2542.798522	22.004275
83.532538	2544.898603	22.009293
83.285160	2541.254242	22.014311
83.571309	2535.677384	22.019328
83.580992	2532.393816	22.024346
83.466312	2538.029594	22.029363
83.190723	2544.173298	22.034381
83.315068	2539.820921	22.039399
83.318772	2548.711067	22.044416
83.625435	2559.438196	22.049434
83.623698	2568.941468	22.054451
83.902032	2566.158903	22.059469
83.619186	2569.059349	22.064487
83.814492	2575.742018	22.069504
83.979374	2581.662510	22.074522
84.191738	2592.735724	22.079539
84.234699	2595.844242	22.084557
84.329559	2592.919814	22.089575
84.220931	2593.511327	22.094592
84.898470	2603.735739	22.099610
84.897533	2617.628957	22.104627
84.866625	2614.449531	22.109645
85.167579	2616.062952	22.114663
84.610182	2615.493483	22.119680
85.220679	2613.694375	22.124698
84.943319	2612.891944	22.129715
85.076279	2614.417904	22.134733
85.091728	2610.726295	22.139751
85.358021	2624.543195	22.144768
85.754586	2635.597225	22.149786
85.601455	2640.478416	22.154803
85.491984	2648.101723	22.159821
85.814435	2641.165239	22.164839
85.747685	2647.203874	22.169856
85.956029	2634.661093	22.174874
85.949197	2642.161112	22.179891
86.084004	2641.275570	22.184909
85.905850	2642.720573	22.189927
85.915898	2664.808359	22.194944
86.324102	2659.004161	22.199962
86.191840	2662.364051	22.204979
86.235559	2660.107188	22.209997
86.176582	2667.072496	22.215015
86.030714	2679.675412	22.220032
86.848436	2676.954029	22.225050
86.666916	2684.702187	22.230067
86.634678	2683.113604	22.235085
86.813918	2691.556737	22.240103
86.907553	2702.850491	22.245120
87.426549	2694.955507	22.250138
87.441269	2702.136590	22.255155
87.907150	2696.506452	22.260173
87.900490	2699.382854	22.265191
87.477074	2700.812395	22.270208
87.705342	2688.001365	22.275226
87.857143	2688.429249	22.280243
88.016834	2691.904648	22.285261
88.289200	2697.647485	22.290279
88.136969	2694.307040	22.295296
88.301942	2681.013526	22.300314
88.459385	2684.492430	22.305331
88.358753	2682.134952	22.310349
88.523206	2676.943100	22.315367
88.402384	2683.091160	22.320384
88.718223	2688.745169	22.325402
89.107820	2701.125865	22.330419
89.066362	2694.659462	22.335437
88.967322	2672.860477	22.340455
88.825298	2677.127675	22.345472
88.898147	2676.299120	22.350490
88.965617	2690.506816	22.355507
89.461289	2700.390342	22.360525
89.506855	2700.004724	22.365543
89.514394	2701.010534	22.370560
89.846634	2705.955039	22.375578
89.423160	2704.070734	22.380595
89.660505	2698.138479	22.385613
89.520382	2698.176279	22.390631
89.722346	2705.675377	22.395648
89.424609	2693.627947	22.400666
89.548016	2699.504439	22.405683
89.427644	2719.725279	22.410701
90.276650	2720.142450	22.415719
90.282932	2731.790677	22.420736
90.380318	2730.664786	22.425754
89.937930	2727.457879	22.430771
89.940584	2723.686182	22.435789
90.637873	2736.167331	22.440807
91.032399	2746.186560	22.445824
90.789304	2738.877306	22.450842
90.887971	2746.528214	22.455859
90.693533	2754.003836	22.460877
90.827100	2749.829868	22.465895
90.550197	2751.520646	22.470912
90.826764	2761.491972	22.475930
91.098770	2760.474602	22.480947
91.118607	2772.398479	22.485965
91.322384	2760.228736	22.490983
91.515473	2776.282175	22.496000
91.564008	2788.141629	22.501018
92.009839	2793.535571	22.506035
92.028311	2799.845035	22.511053
92.235019	2790.373255	22.516071
92.155831	2788.552112	22.521088
92.062432	2792.691836	22.526106
92.677963	2792.851846	22.531123
92.115759	2792.226310	22.536141
92.503632	2784.537909	22.541159
92.565148	2787.122821	22.546176
92.574315	2790.435467	22.551194
92.550378	2788.290115	22.556211
92.484557	2803.377104	22.561229
93.016205	2806.147619	22.566247
92.378091	2812.723430	22.571264
93.113398	2816.147106	22.576282
93.043433	2807.860891	22.581299
92.946017	2812.973316	22.586317
93.264863	2812.201136	22.591335
93.098687	2820.268882	22.596352
93.300620	2823.557834	22.601370
93.659200	2824.613146	22.606387
93.519851	2827.374516	22.611405
93.837671	2830.153079	22.616423
93.464737	2835.207412	22.621440
93.555895	2842.903715	22.626458
94.083013	2851.532622	22.631475
94.151214	2850.161937	22.636493
94.439034	2851.969946	22.641511
94.505070	2842.093970	22.646528
94.454970	2844.992939	22.651546
94.309581	2854.487167	22.656563
94.197369	2868.224320	22.661581
94.761064	2862.749329	22.666599
95.106653	2865.829714	22.671616
94.989118	2875.237558	22.676634
95.112122	2871.443936	22.681651
95.070752	2868.007295	22.686669
95.586219	2866.784742	22.691687
95.476522	2865.650055	22.696704
95.539044	2866.653625	22.701722
95.383377	2868.675864	22.706739
95.053115	2862.828772	22.711757
95.462549	2876.639361	22.716775
95.326294	2890.967306	22.721792
95.447976	2892.169968	22.726810
95.241135	2886.149005	22.731827
95.437577	2900.210544	22.736845
96.357630	2905.988319	22.741863
96.345646	2914.164657	22.746880
96.832382	2914.145887	22.751898
96.950980	2904.618331	22.756915
96.536363	2904.885077	22.761933
96.880973	2904.367682	22.766951
96.987777	2904.310227	22.771968
96.815523	2896.929913	22.776986
96.788502	2897.098440	22.782003
96.582395	2910.357894	22.787021
96.773210	2914.068353	22.792039
97.217404	2931.531480	22.797056
97.360828	2929.047601	22.802074
97.455087	2927.335151	22.807091
97.153581	2931.788201	22.812109
97.064219	2925.281832	22.817127
97.438341	2934.632096	22.822144
97.709943	2947.492123	22.827162
98.202326	2951.161950	22.832179
98.165076	2949.324793	22.837197
98.278452	2950.030090	22.842215
98.423904	2946.485445	22.847232
98.231008	2942.520065	22.852250
98.714953	2938.465086	22.857267
98.478577	2933.316631	22.862285
98.811726	2927.060088	22.867303
98.810468	2933.252739	22.872320
98.493025	2936.414273	22.877338
98.657671	2949.464540	22.882355
98.640244	2957.401881	22.887373
98.886277	2960.431504	22.892391
99.065496	2968.082590	22.897408
98.853915	2962.762992	22.902426
99.504417	2978.170986	22.907443
99.575476	2992.911744	22.912461
99.430983	2991.618349	22.917479
99.384380	2984.739193	22.922496
99.382958	2997.250408	22.927514
99.691067	2997.006962	22.932531
99.709346	3016.325995	22.937549
99.838566	3009.520451	22.942567
99.885795	3021.216144	22.947584
100.123344	3015.542554	22.952602
100.076997	3016.067575	22.957619
100.510430	3031.749275	22.962637
100.503532	3031.463346	22.967655
100.521132	3035.882519	22.972672
100.777100	3043.221857	22.977690
100.830628	3035.474941	22.982707
100.674646	3040.470304	22.987725
101.469266	3051.557300	22.992743
101.153000	3053.213205	22.997760
101.271087	3062.041611	23.002778
101.384962	3051.268048	23.007795
101.268178	3054.887558	23.012813
101.362163	3058.862457	23.017831
101.264241	3063.053445	23.022848
101.392042	3058.018684	23.027866
101.928773	3067.788713	23.032883
102.420800	3072.620071	23.037901
102.532234	3064.804161	23.042919
102.512831	3069.633086	23.047936
102.442363	3066.409242	23.052954
103.106617	3065.677957	23.057971
102.514913	3059.808383	23.062989
102.500427	3041.966178	23.068007
102.802836	3061.689191	23.073024
102.492119	3056.949945	23.078042
102.626757	3061.133130	23.083059
102.713289	3063.969833	23.088077
102.555028	3065.604295	23.093095
102.616104	3081.700654	23.098112
103.152868	3082.639868	23.103130
103.082552	3085.529399	23.108147
103.170353	3087.968237	23.113165
103.362519	3109.100315	23.118183
103.657602	3109.890948	23.123200
103.315037	3118.137784	23.128218
104.181663	3109.323718	23.133235
103.644271	3117.629292	23.138253
103.668384	3120.573561	23.143271
104.046259	3126.293798	23.148288
103.934947	3135.868084	23.153306
104.646437	3141.230239	23.158323
104.385458	3138.844012	23.163341
104.295587	3144.046883	23.168359
104.969455	3150.841469	23.173376
104.730700	3161.133116	23.178394
105.140725	3155.401068	23.183411
104.896077	3149.878258	23.188429
104.957434	3164.128311	23.193447
105.044377	3157.802713	23.198464
105.531568	3177.885288	23.203482
105.693108	3177.689909	23.208499
105.792191	3184.738117	23.213517
105.875931	3178.400386	23.218535
106.108315	3171.733369	23.223552
105.787954	3177.069975	23.228570
106.308822	3172.163352	23.233587
106.201911	3175.285837	23.238605
106.241537	3170.741349	23.243623
106.156410	3176.723056	23.248640
106.275710	3176.499536	23.253658
106.495002	3182.752619	23.258675
106.445339	3203.811995	23.263693
106.682648	3205.482722	23.268711
106.939489	3199.967034	23.273728
106.842978	3203.684415	23.278746
106.887341	3201.645156	23.283763
106.798385	3214.643572	23.288781
107.015155	3224.015330	23.293799
107.233497	3223.397652	23.298816
107.266892	3230.673879	23.303834
107.410179	3229.761741	23.308851
107.544457	3247.721601	23.313869
107.650148	3254.393226	23.318887
107.719958	3254.950667	23.323904
107.638877	3251.340235	23.328922
108.028932	3260.315763	23.333939
108.262859	3270.679062	23.338957
108.147533	3268.592067	23.343975
108.353480	3272.656890	23.348992
108.379599	3275.657684	23.354010
108.354122	3263.106683	23.359027
108.325530	3280.107215	23.364045
108.521665	3291.600000	23.369063
108.946466	3290.994361	23.374080
109.033979	3304.069519	23.379098
109.331480	3292.765393	23.384115
109.104613	3298.311566	23.389133
108.831722	3299.626187	23.394151
109.556786	3316.600942	23.399168
109.690714	3322.214039	23.404186
109.951238	3321.536136	23.409203
109.775448	3317.138771	23.414221
110.446369	3320.881875	23.419239
110.262814	3318.748687	23.424256
109.869018	3329.733674	23.429274
109.989654	3317.002079	23.434291
110.186877	3334.879635	23.439309
110.443267	3329.420789	23.444327
110.825201	3336.677512	23.449344
110.628476	3356.390187	23.454362
110.704871	3342.709144	23.459379
110.967627	3339.496493	23.464397
110.660430	3347.157192	23.469415
111.260907	3362.352374	23.474432
110.972902	3372.923240	23.479450
111.265915	3367.818484	23.484467
111.226853	3366.606487	23.489485
111.504890	3379.046052	23.494503
111.732803	3387.753365	23.499520
111.619743	3398.246509	23.504538
111.991758	3392.182593	23.509555
111.745427	3398.779677	23.514573
111.941678	3392.503257	23.519591
112.102725	3406.999944	23.524608
112.067283	3427.429287	23.529626
112.085808	3421.013251	23.534643
112.775776	3428.828039	23.539661
112.552512	3439.354146	23.544679
112.785007	3437.828433	23.549696
112.684914	3449.559967	23.554714
113.010352	3444.440672	23.559731
113.279765	3444.607237	23.564749
113.390821	3447.402308	23.569767
113.640030	3450.750295	23.574784
113.497134	3462.075041	23.579802
113.977787	3458.689571	23.584819
114.016039	3464.383889	23.589837
113.786422	3456.163262	23.594855
114.106473	3453.904307	23.599872
113.932489	3455.086761	23.604890
114.097650	3461.357837	23.609907
114.511261	3468.391905	23.614925
114.110218	3479.946225	23.619943
114.526740	3481.800541	23.624960
114.722369	3492.608640	23.629978
114.816513	3479.376065	23.634995
114.879017	3475.506519	23.640013
114.925866	3476.417878	23.645031
114.974154	3487.072168	23.650048
115.112277	3501.206381	23.655066
115.436209	3502.103008	23.660083
115.566026	3500.113535	23.665101
115.670460	3512.302476	23.670119
115.807401	3505.265140	23.675136
115.562223	3514.895188	23.680154
115.650609	3516.175669	23.685171
116.069302	3517.546753	23.690189
116.131239	3519.734025	23.695207
116.319578	3519.020010	23.700224
116.022837	3524.368822	23.705242
116.287899	3522.976905	23.710259
116.631331	3535.797765	23.715277
116.158866	3546.406919	23.720295
116.294021	3545.297191	23.725312
116.446591	3553.858504	23.730330
116.719201	3563.903485	23.735347
116.610920	3568.897880	23.740365
117.101893	3577.409674	23.745383
117.202774	3573.385790	23.750400
117.133799	3595.622738	23.755418
117.690434	3592.632565	23.760435
117.624117	3595.430025	23.765453
117.739748	3598.066596	23.770471
118.240421	3601.306023	23.775488
118.401714	3608.259495	23.780506
118.680763	3621.264031	23.785523
118.544142	3623.027735	23.790541
118.541832	3623.621665	23.795559
118.748496	3616.431401	23.800576
119.035102	3611.327575	23.805594
118.771136	3617.873828	23.810611
119.016473	3605.229926	23.815629
118.664541	3613.541569	23.820647
118.712727	3621.194397	23.825664
118.702075	3628.629142	23.830682
118.816547	3648.347340	23.835699
119.126258	3644.319333	23.840717
119.289916	3654.889479	23.845735
119.889045	3660.853187	23.850752
119.693941	3661.900069	23.855770
119.774232	3665.681548	23.860787
120.159792	3670.002556	23.865805
120.333833	3686.981392	23.870823
120.705176	3682.508221	23.875840
120.687534	3689.802049	23.880858
120.815085	3689.785550	23.885875
120.674282	3686.001268	23.890893
120.698077	3687.661096	23.895911
120.872771	3690.496796	23.900928
120.903107	3695.766329	23.905946
120.856181	3699.791714	23.910963
121.496490	3704.069912	23.915981
120.981884	3714.205979	23.920999
121.352728	3723.787570	23.926016
121.235948	3733.151557	23.931034
121.826329	3736.509604	23.936051
121.492817	3745.629592	23.941069
121.515599	3756.591011	23.946087
121.817802	3754.322173	23.951104
122.422675	3767.427585	23.956122
122.812994	3775.721583	23.961139
123.230038	3781.918837	23.966157
123.173901	3780.188691	23.971175
122.953926	3776.410404	23.976192
123.068350	3778.258130	23.981210
123.100636	3774.061819	23.986227
123.303217	3774.620699	23.991245
123.367500	3780.251095	23.996263
123.367259	3774.137698	24.001280
123.062199	3783.051276	24.006298
123.363324	3794.711098	24.011315
123.527603	3799.123402	24.016333
123.619050	3800.280334	24.021351
123.763439	3806.602109	24.026368
123.957846	3832.282836	24.031386
123.795805	3823.256146	24.036403
124.457704	3824.598857	24.041421
124.304500	3827.425662	24.046439
124.659239	3843.338105	24.051456
124.811582	3842.525526	24.056474
124.483192	3854.015117	24.061491
124.964027	3830.208602	24.066509
125.151925	3850.294339	24.071527
125.122186	3840.697853	24.076544
125.385833	3859.278900	24.081562
125.554462	3868.260802	24.086579
125.832620	3867.236102	24.091597
125.724622	3878.287393	24.096615
125.886662	3873.060855	24.101632
125.929732	3865.485650	24.106650
125.931503	3869.471928	24.111667
126.472947	3878.297946	24.116685
126.520691	3892.187724	24.121703
126.205862	3892.385288	24.126720
126.395319	3890.096112	24.131738
126.451642	3888.967073	24.136755
127.051362	3899.999723	24.141773
127.038249	3909.360286	24.146791
127.173632	3909.519317	24.151808
127.433978	3921.870480	24.156826
127.203008	3909.474118	24.161843
127.609283	3901.280535	24.166861
127.502266	3921.923582	24.171879
127.645536	3927.065130	24.176896
127.803280	3927.653089	24.181914
127.805916	3927.340411	24.186931
128.210846	3930.613744	24.191949
128.383339	3963.327078	24.196967
128.250795	3960.560928	24.201984
128.607607	3950.089883	24.207002
128.781003	3962.382017	24.212019
128.879235	3947.620826	24.217037
128.974554	3960.723651	24.222055
129.178247	3970.195679	24.227072
129.219856	3982.877629	24.232090
129.181154	3983.931742	24.237107
129.478127	3976.739900	24.242125
129.528283	3977.461393	24.247143
129.700006	3993.531871	24.252160
129.924339	4011.368002	24.257178
129.805396	4015.631922	24.262195
129.923272	4015.932557	24.267213
129.968739	4019.400747	24.272231
130.238723	4026.176487	24.277248
130.369212	4031.421056	24.282266
130.269675	4033.248463	24.287283
130.733104	4037.434342	24.292301
131.021051	4052.792395	24.297319
131.113935	4048.728619	24.302336
131.095515	4047.519675	24.307354
130.753110	4051.284982	24.312371
131.361221	4057.329488	24.317389
131.587938	4074.682398	24.322407
131.690892	4081.077002	24.327424
131.778767	4072.907663	24.332442
131.739261	4075.142359	24.337459
132.401337	4069.979946	24.342477
132.145287	4074.565074	24.347495
132.179582	4087.753244	24.352512
132.310183	4089.781548	24.357530
132.216347	4096.039513	24.362547
132.548177	4092.538221	24.367565
132.946419	4110.918663	24.372583
133.135471	4116.087857	24.377600
133.641619	4104.605550	24.382618
133.303668	4117.214125	24.387635
133.555321	4115.297149	24.392653
133.321833	4117.123326	24.397671
133.490343	4109.026637	24.402688
133.689920	4114.115283	24.407706
133.643450	4136.267329	24.412723
134.098971	4138.096705	24.417741
134.106774	4142.858555	24.422759
133.894427	4144.340563	24.427776
133.993172	4141.610970	24.432794
134.260642	4159.415281	24.437811
134.511817	4167.873158	24.442829
134.335048	4170.523775	24.447847
134.648927	4178.110222	24.452864
135.081031	4177.134132	24.457882
135.126892	4186.662410	24.462899
135.455111	4181.832856	24.467917
135.803401	4188.217708	24.472935
135.623680	4207.041740	24.477952
135.966139	4206.900248	24.482970
136.025357	4214.324355	24.487987
136.251094	4211.606543	24.493005
136.348252	4212.267071	24.498023
136.348014	4206.576474	24.503040
136.354381	4213.781554	24.508058
136.140428	4226.815940	24.513075
136.754843	4235.908529	24.518093
136.643449	4233.839748	24.523111
137.098682	4243.534731	24.528128
137.440168	4251.763957	24.533146
137.009627	4256.313171	24.538163
137.557186	4256.395408	24.543181
137.505441	4254.645595	24.548199
137.320562	4263.881580	24.553216
137.812083	4266.911082	24.558234
137.550619	4283.806779	24.563251
137.779085	4280.343639	24.568269
137.933681	4287.885493	24.573287
138.255900	4298.702774	24.578304
138.658244	4305.480106	24.583322
138.554705	4315.088526	24.588339
138.292073	4307.573356	24.593357
138.557101	4322.572228	24.598375
138.650122	4334.930787	24.603392
138.971757	4335.578465	24.608410
139.142342	4357.577046	24.613427
139.293923	4350.395068	24.618445
139.627557	4358.073205	24.623463
139.829288	4365.929700	24.628480
140.516040	4374.812247	24.633498
140.110781	4382.280332	24.638515
140.651973	4369.220542	24.643533
140.491625	4374.327424	24.648551
140.343069	4372.753646	24.653568
140.718053	4380.763084	24.658586
140.678630	4383.253469	24.663603
140.753738	4390.997121	24.668621
141.025039	4397.952708	24.673639
140.857799	4402.075890	24.678656
141.406279	4401.406774	24.683674
141.361154	4422.151228	24.688691
141.423555	4417.006331	24.693709
141.675121	4423.415795	24.698727
141.689085	4425.699023	24.703744
141.834918	4436.221901	24.708762
142.191603	4447.665176	24.713779
142.006973	4453.826927	24.718797
142.114682	4448.798065	24.723815
142.017980	4460.564446	24.728832
142.458706	4463.349380	24.733850
142.388263	4474.597195	24.738867
142.417133	4481.306486	24.743885
142.844509	4497.312357	24.748903
143.054281	4486.737642	24.753920
143.381620	4498.674755	24.758938
143.131614	4513.611936	24.763955
143.529042	4519.755684	24.768973
143.708127	4516.205496	24.773991
143.708029	4528.424023	24.779008
144.232970	4536.331274	24.784026
143.821823	4555.131727	24.789043
144.229978	4551.807847	24.794061
144.337674	4570.773734	24.799079
144.594474	4575.496931	24.804096
144.822656	4570.906953	24.809114
144.721599	4581.537794	24.814131
145.186645	4577.422270	24.819149
145.612215	4591.487332	24.824167
145.655452	4605.842348	24.829184
146.062124	4599.501188	24.834202
145.864650	4603.095693	24.839219
145.996161	4600.326210	24.844237
146.162642	4595.666923	24.849255
145.917986	4603.106936	24.854272
146.417668	4604.623317	24.859290
146.514347	4616.523823	24.864307
146.553596	4616.599981	24.869325
146.893393	4610.266072	24.874343
146.836321	4615.738865	24.879360
146.869680	4625.455547	24.884378
146.959826	4632.875010	24.889395
146.854849	4638.503618	24.894413
147.316112	4637.898576	24.899431
147.169197	4654.432738	24.904448
147.502034	4660.949576	24.909466
147.719091	4679.043166	24.914483
147.685294	4684.405038	24.919501
147.726330	4697.169644	24.924519
148.377139	4712.298161	24.929536
148.339971	4714.983937	24.934554
148.612169	4722.520288	24.939571
148.710631	4725.718381	24.944589
149.100343	4734.050794	24.949607
149.172241	4733.885139	24.954624
149.332303	4740.570944	24.959642
149.306678	4730.869184	24.964659
149.345420	4744.587415	24.969677
149.912317	4742.656014	24.974695
149.690138	4764.410068	24.979712
149.778984	4757.098815	24.984730
150.354139	4781.026618	24.989747
150.554656	4785.768102	24.994765
150.677451	4780.108673	24.999783
150.507076	4789.200628	25.004800
150.542234	4788.257901	25.009818
151.154291	4794.882824	25.014835
151.009971	4804.507321	25.019853
150.984164	4808.652764	25.024871
151.094256	4819.837965	25.029888
150.897879	4817.378325	25.034906
151.528846	4828.769669	25.039923
151.592985	4835.135863	25.044941
151.795519	4841.411070	25.049959
152.124699	4858.682495	25.054976
152.501317	4846.777988	25.059994
152.528570	4858.651586	25.065011
152.449690	4862.369717	25.070029
152.627548	4857.222501	25.075047
152.410290	4863.992349	25.080064
152.808966	4877.736709	25.085082
153.204666	4884.808843	25.090099
152.852638	4884.844915	25.095117
153.661790	4891.909496	25.100135
153.576841	4904.554980	25.105152
153.607121	4908.234030	25.110170
153.786897	4905.460143	25.115187
153.909141	4920.806855	25.120205
154.205303	4922.588526	25.125223
154.195567	4933.966057	25.130240
154.191458	4928.954471	25.135258
154.413658	4943.840581	25.140275
154.572974	4958.019981	25.145293
155.116442	4946.480832	25.150311
155.003806	4961.428557	25.155328
155.406887	4983.707346	25.160346
155.692110	4981.049602	25.165363
155.475842	4988.614767	25.170381
155.923426	4983.094094	25.175399
156.048687	4988.986827	25.180416
156.269861	5001.862486	25.185434
155.999828	5001.608024	25.190451
156.155416	5000.346673	25.195469
156.603596	5006.264891	25.200487
156.712942	5011.888654	25.205504
156.893552	5015.582199	25.210522
157.177606	5019.976155	25.215539
157.014076	5024.569211	25.220557
157.404579	5033.491896	25.225575
157.359426	5053.429023	25.230592
157.301221	5045.540820	25.235610
158.044146	5060.974090	25.240627
157.845251	5068.457672	25.245645
157.995627	5067.351795	25.250663
158.223446	5068.225590	25.255680
158.818763	5070.926579	25.260698
159.038042	5071.763827	25.265715
159.132831	5073.330661	25.270733
159.872062	5063.424417	25.275751
159.803220	5079.375490	25.280768
159.514290	5076.459911	25.285786
159.770845	5073.793990	25.290803
159.450656	5070.690734	25.295821
159.927983	5077.182071	25.300839
159.752514	5087.458643	25.305856
159.865217	5102.636545	25.310874
160.084046	5100.948687	25.315891
159.725561	5108.308778	25.320909
160.329396	5122.018226	25.325927
160.251536	5130.325768	25.330944
160.331069	5144.643994	25.335962
161.023680	5151.799422	25.340979
160.803920	5156.278163	25.345997
161.255548	5173.941167	25.351015
161.428632	5183.708993	25.356032
161.176616	5185.071000	25.361050
161.771661	5195.398121	25.366067
161.485562	5202.434487	25.371085
162.069935	5206.286163	25.376103
162.240915	5230.107036	25.381120
162.656417	5233.568352	25.386138
162.728553	5238.715035	25.391155
162.848165	5243.286160	25.396173
162.603990	5241.162179	25.401191
162.976061	5256.369270	25.406208
163.054412	5253.579557	25.411226
163.331255	5255.932439	25.416243
163.031945	5257.071390	25.421261
163.455152	5274.660005	25.426279
163.826855	5283.115422	25.431296
164.001676	5284.063766	25.436314
164.442161	5292.994580	25.441331
164.532733	5297.652308	25.446349
164.793012	5302.106852	25.451367
164.811502	5306.469624	25.456384
164.893227	5312.340832	25.461402
165.007907	5304.308809	25.466419
164.539682	5325.678870	25.471437
164.959266	5333.826987	25.476455
165.046480	5335.997917	25.481472
165.112315	5354.175699	25.486490
165.689722	5359.139585	25.491507
165.707400	5381.390484	25.496525
165.844650	5383.007552	25.501543
166.009635	5391.861360	25.506560
166.251592	5407.922158	25.511578
166.396541	5408.909881	25.516595
167.016561	5404.631159	25.521613
167.853259	5394.390753	25.526631
168.163046	5401.280761	25.531648
168.282228	5397.304129	25.536666
168.646668	5388.844932	25.541683
168.166157	5385.971756	25.546701
168.470550	5382.250378	25.551719
168.440589	5376.292581	25.556736
168.608462	5391.572612	25.561754
169.051891	5388.217839	25.566771
168.853562	5393.261476	25.571789
169.294653	5395.225805	25.576807
169.171155	5392.713705	25.581824
169.242167	5395.190191	25.586842
169.259300	5394.992022	25.591859
169.556332	5408.563220	25.596877
169.557747	5414.974104	25.601895
169.837156	5421.202822	25.606912
169.753939	5427.589009	25.611930
170.070839	5434.812514	25.616947
169.934450	5453.375411	25.621965
170.042615	5448.106305	25.626983
170.422373	5460.594599	25.632000
170.317702	5476.930382	25.637018
170.889508	5473.009525	25.642035
170.997652	5490.896768	25.647053
170.963453	5497.909813	25.652071
171.438435	5508.934462	25.657088
171.571494	5526.218118	25.662106
171.670785	5525.000219	25.667123
171.843922	5528.688719	25.672141
171.734122	5539.015295	25.677159
171.891385	5551.336272	25.682176
172.272195	5560.658452	25.687194
172.398360	5572.469768	25.692212
172.404184	5590.395135	25.697229
172.512239	5585.776257	25.702247
173.092728	5603.883631	25.707264
172.971667	5611.260620	25.712282
173.499716	5620.389453	25.717300
173.711421	5629.987365	25.722317
174.082133	5629.977200	25.727335
174.392684	5624.016812	25.732352
174.517223	5625.598002	25.737370
174.617557	5627.435486	25.742388
174.775712	5635.624442	25.747405
175.027109	5648.880955	25.752423
175.094305	5643.368803	25.757440
175.257898	5648.602374	25.762458
175.629432	5642.244228	25.767476
175.763572	5634.900318	25.772493
175.398063	5639.982676	25.777511
175.767591	5644.915876	25.782528
175.764759	5669.452517	25.787546
176.144482	5669.620874	25.792564
175.777178	5668.876494	25.797581
176.124270	5685.293644	25.802599
176.550338	5701.070354	25.807616
176.509617	5709.568085	25.812634
176.917571	5719.624760	25.817652
176.912770	5735.901034	25.822669
177.089053	5737.158520	25.827687
177.031744	5742.874745	25.832704
177.490767	5752.244822	25.837722
177.571809	5761.635872	25.842740
177.763615	5764.380852	25.847757
177.696260	5777.775470	25.852775
178.115566	5789.105677	25.857792
178.162752	5795.364366	25.862810
178.420890	5810.558095	25.867828
178.411510	5823.362907	25.872845
178.556352	5826.080485	25.877863
179.058769	5837.277832	25.882880
179.397854	5847.035953	25.887898
179.267610	5856.718789	25.892916
180.086732	5867.611163	25.897933
179.791217	5869.027341	25.902951
180.338428	5881.606647	25.907968
180.705420	5890.132527	25.912986
180.833928	5900.264375	25.918004
180.775386	5895.175769	25.923021
180.794186	5902.559510	25.928039
181.333694	5914.069948	25.933056
181.486861	5921.757908	25.938074
181.686714	5913.339877	25.943092
181.114868	5920.563054	25.948109
181.743988	5940.342511	25.953127
182.075112	5934.997516	25.958144
181.857255	5953.387365	25.963162
182.389334	5959.213919	25.968180
182.826739	5963.047604	25.973197
182.466569	5973.050395	25.978215
182.949197	5981.040628	25.983232
182.872722	5998.332101	25.988250
183.151015	6007.260110	25.993268
183.735272	6019.821119	25.998285
183.734095	6018.789287	26.003303
183.701500	6018.523094	26.008320
183.972033	6037.622991	26.013338
184.088416	6045.468248	26.018356
184.473121	6041.699511	26.023373
184.756592	6061.892771	26.028391
184.998246	6067.265827	26.033408
185.097730	6080.659946	26.038426
185.223844	6078.462432	26.043444
185.235176	6074.243600	26.048461
185.187988	6089.892304	26.053479
185.423153	6099.682524	26.058496
185.767762	6115.753218	26.063514
186.132720	6126.012524	26.068532
186.117860	6123.237190	26.073549
186.345685	6134.224941	26.078567
186.409393	6145.544444	26.083584
186.434994	6147.889210	26.088602
186.809335	6154.368560	26.093620
187.303075	6169.693209	26.098637
187.317993	6173.071869	26.103655
187.288076	6169.373972	26.108672
187.287161	6182.158778	26.113690
187.560295	6194.995625	26.118708
187.975083	6192.074472	26.123725
187.614458	6211.743159	26.128743
188.089441	6216.855809	26.133760
188.143467	6235.339348	26.138778
188.653955	6248.211883	26.143796
188.638265	6259.509095	26.148813
188.766912	6275.581987	26.153831
189.104142	6280.523546	26.158848
189.202950	6299.767249	26.163866
189.502435	6307.426279	26.168884
189.505606	6316.318357	26.173901
190.165688	6329.881069	26.178919
189.932914	6334.851410	26.183936
190.079619	6351.410842	26.188954
190.688321	6355.151652	26.193972
191.227145	6357.811127	26.198989
191.447249	6380.401061	26.204007
191.710055	6379.874217	26.209024
191.906623	6383.827562	26.214042
191.853365	6369.659355	26.219060
192.095502	6384.145797	26.224077
192.135367	6397.776712	26.229095
192.354024	6403.355477	26.234112
192.497292	6406.673160	26.239130
192.786760	6412.114635	26.244148
192.939034	6422.249386	26.249165
192.545859	6439.577957	26.254183
192.887360	6433.634586	26.259200
193.238604	6450.588418	26.264218
193.211950	6467.118126	26.269236
193.723424	6478.901607	26.274253
193.969979	6496.541003	26.279271
194.137752	6487.881480	26.284288
194.381752	6503.355778	26.289306
194.550456	6508.459375	26.294324
194.795035	6525.129996	26.299341
194.777574	6526.483992	26.304359
195.502204	6528.499005	26.309376
195.515340	6529.450492	26.314394
195.823589	6551.278772	26.319412
196.092226	6552.373570	26.324429
195.969155	6560.745622	26.329447
196.071951	6558.109741	26.334464
196.358958	6574.262412	26.339482
196.437295	6579.020232	26.344500
196.849755	6578.438515	26.349517
197.115689	6586.652156	26.354535
197.151974	6586.040618	26.359552
197.277490	6601.965918	26.364570
197.516215	6611.945263	26.369588
197.596812	6619.887884	26.374605
197.838435	6633.061403	26.379623
198.144121	6640.972147	26.384640
198.400990	6657.902984	26.389658
198.584843	6659.686532	26.394676
198.972130	6669.645935	26.399693
198.794561	6676.561796	26.404711
199.043395	6684.519291	26.409728
199.247955	6693.266555	26.414746
199.656462	6707.023397	26.419764
199.676985	6700.905784	26.424781
199.264772	6713.259387	26.429799
199.975947	6722.309756	26.434816
200.541783	6729.649701	26.439834
200.661574	6730.916052	26.444852
201.184558	6731.706096	26.449869
200.958518	6741.161244	26.454887
201.528197	6746.170912	26.459904
201.271928	6758.288764	26.464922
201.160593	6744.896400	26.469940
201.539092	6755.532764	26.474957
201.584230	6770.394270	26.479975
202.084552	6778.839830	26.484992
202.233268	6784.546402	26.490010
202.323991	6798.785266	26.495028
203.141122	6798.658250	26.500045
202.911343	6811.734825	26.505063
203.437903	6815.658985	26.510080
203.526153	6820.289054	26.515098
203.529547	6818.460959	26.520116
203.658207	6825.111383	26.525133
203.764059	6835.420900	26.530151
204.232046	6831.487512	26.535168
204.483011	6846.329662	26.540186
204.711604	6858.608849	26.545204
204.830479	6856.358705	26.550221
205.013783	6871.454481	26.555239
205.107801	6884.884764	26.560256
205.546381	6894.176538	26.565274
205.482725	6895.446207	26.570292
205.688387	6905.213041	26.575309
205.831749	6924.630402	26.580327
206.198837	6928.781450	26.585344
206.592396	6942.711264	26.590362
206.704788	6949.149603	26.595380
206.900921	6942.442660	26.600397
206.843556	6971.585824	26.605415
207.229409	6967.965090	26.610432
207.378014	6980.967092	26.615450
207.550646	6985.514615	26.620468
207.749795	6996.538917	26.625485
207.593385	7014.206827	26.630503
207.970830	7020.127248	26.635520
208.329900	7040.107784	26.640538
208.596865	7046.935634	26.645556
208.899741	7051.084080	26.650573
208.790201	7067.270513	26.655591
208.955479	7073.899542	26.660608
209.524067	7083.707829	26.665626
209.694300	7097.126402	26.670644
209.838126	7105.346660	26.675661
210.181948	7116.657879	26.680679
210.090597	7125.792357	26.685696
210.346087	7139.734347	26.690714
210.431456	7156.338782	26.695732
210.727193	7162.783377	26.700749
211.153303	7175.634980	26.705767
210.990850	7182.479227	26.710784
211.634478	7198.488537	26.715802
211.921982	7208.343810	26.720820
212.161840	7207.744752	26.725837
212.178011	7225.960540	26.730855
212.434058	7233.869799	26.735872
212.997704	7227.894743	26.740890
212.857793	7250.017767	26.745908
212.850871	7242.922468	26.750925
212.944719	7261.195647	26.755943
213.346929	7271.765484	26.760960
213.822872	7278.295710	26.765978
213.699152	7290.727901	26.770996
214.177453	7297.039944	26.776013
214.052259	7302.786165	26.781031
214.679037	7311.628990	26.786048
214.624916	7331.497389	26.791066
214.805460	7324.303421	26.796084
215.242388	7341.011133	26.801101
215.251492	7361.160152	26.806119
215.595642	7358.133011	26.811136
215.617984	7360.367950	26.816154
215.824923	7382.159327	26.821172
216.116977	7383.998709	26.826189
216.335454	7393.419710	26.831207
216.500245	7402.962722	26.836224
216.806373	7420.325401	26.841242
216.888556	7428.539617	26.846260
216.932712	7436.169422	26.851277
217.178107	7454.690691	26.856295
217.390760	7473.406489	26.861312
218.031284	7482.395630	26.866330
217.813708	7495.862244	26.871348
218.291148	7502.632241	26.876365
218.669847	7500.736178	26.881383
218.588404	7520.444877	26.886400
219.108075	7532.666571	26.891418
219.432586	7543.030836	26.896436
219.848091	7539.667397	26.901453
220.267344	7554.714373	26.906471
220.514739	7544.627668	26.911488
220.943998	7549.084867	26.916506
220.983422	7563.398606	26.921524
221.256389	7569.389140	26.926541
221.264861	7577.100324	26.931559
221.277796	7564.755046	26.936576
221.651608	7562.367261	26.941594
221.573091	7586.498387	26.946612
222.316710	7584.346616	26.951629
222.226362	7584.828106	26.956647
222.253560	7605.823782	26.961664
222.461281	7616.433569	26.966682
222.607610	7617.954717	26.971700
222.687995	7629.768175	26.976717
223.051487	7648.883694	26.981735
223.070014	7666.884881	26.986752
223.815803	7665.114751	26.991770
223.944526	7664.387764	26.996788
224.409554	7679.314068	27.001805
224.555778	7694.321587	27.006823
224.608940	7691.863745	27.011840
224.969704	7697.603883	27.016858
225.083703	7711.981893	27.021876
225.182155	7719.132981	27.026893
225.079730	7723.426761	27.031911
225.352932	7744.801009	27.036928
225.717686	7742.777659	27.041946
225.845833	7764.398655	27.046964
226.267354	7761.233126	27.051981
226.293714	7794.184445	27.056999
226.495682	7795.542255	27.062016
227.221876	7806.014606	27.067034
226.721814	7821.397502	27.072052
227.149286	7829.027774	27.077069
227.259374	7846.307727	27.082087
227.595078	7864.070310	27.087104
227.827027	7879.326660	27.092122
228.099943	7892.291012	27.097140
228.139802	7898.886197	27.102157
228.499330	7913.532363	27.107175
228.797137	7919.746445	27.112192
228.977955	7930.439526	27.117210
228.927353	7943.264864	27.122228
229.759564	7958.162641	27.127245
229.834901	7964.023067	27.132263
230.105270	7973.950874	27.137280
230.440571	7972.831819	27.142298
230.255034	7986.634756	27.147316
231.007378	7995.360498	27.152333
230.776655	8010.044968	27.157351
230.993970	8018.610932	27.162368
231.532765	8031.404551	27.167386
231.384999	8045.877245	27.172404
231.743459	8052.609144	27.177421
232.210384	8063.137793	27.182439
231.997815	8074.053209	27.187456
232.462492	8076.449828	27.192474
232.394967	8095.500322	27.197492
232.969702	8107.284477	27.202509
233.104800	8122.720272	27.207527
233.143107	8144.838721	27.212544
233.493465	8138.025252	27.217562
233.829729	8166.250321	27.222580
234.100234	8179.770883	27.227597
234.610335	8185.314289	27.232615
234.642694	8193.422952	27.237632
234.600267	8204.239344	27.242650
234.522130	8217.110200	27.247668
235.258088	8231.881120	27.252685
235.315472	8233.829736	27.257703
236.031248	8248.505944	27.262720
236.265828	8251.244641	27.267738
236.570240	8280.238841	27.272756
236.912946	8285.315845	27.277773
237.217801	8292.232971	27.282791
237.062054	8307.029128	27.287808
237.606289	8309.618598	27.292826
237.485119	8325.485931	27.297844
237.550347	8336.582401	27.302861
238.238112	8348.851082	27.307879
238.317116	8357.659729	27.312896
238.521828	8369.612158	27.317914
238.682687	8383.418287	27.322932
238.678955	8394.345577	27.327949
239.319367	8407.338316	27.332967
239.542637	8431.205726	27.337984
239.549832	8434.623888	27.343002
239.806996	8458.785976	27.348020
240.004299	8466.717541	27.353037
240.320037	8476.499645	27.358055
240.295129	8499.805942	27.363072
241.268857	8501.103635	27.368090
241.101500	8510.212747	27.373108
241.299785	8519.823737	27.378125
241.809048	8536.502333	27.383143
242.018474	8549.524388	27.388160
242.685803	8563.087633	27.393178
242.188836	8573.485663	27.398196
242.359451	8583.202019	27.403213
242.541608	8591.887379	27.408231
243.013320	8607.024920	27.413248
243.516401	8623.016314	27.418266
243.530976	8634.796464	27.423284
243.512951	8648.403332	27.428301
244.171512	8654.678310	27.433319
243.898102	8667.567253	27.438336
243.850295	8678.861480	27.443354
244.800151	8695.825219	27.448372
244.768247	8707.644222	27.453389
245.085721	8723.604616	27.458407
245.422810	8739.088406	27.463424
245.556399	8736.365336	27.468442
246.139713	8749.054654	27.473460
246.105621	8761.609636	27.478477
246.153986	8766.830469	27.483495
246.103460	8786.131596	27.488512
246.554228	8789.221882	27.493530
246.894258	8813.602002	27.498548
247.528969	8835.271672	27.503565
247.624073	8835.440181	27.508583
247.721310	8856.821014	27.513600
248.133155	8868.608919	27.518618
248.455685	8882.175567	27.523636
248.218272	8897.354292	27.528653
249.075368	8902.474511	27.533671
249.172681	8922.207389	27.538688
249.487198	8931.462684	27.543706
249.905207	8955.982394	27.548724
249.731456	8956.451646	27.553741
250.031320	8961.829121	27.558759
250.546687	8987.972268	27.563776
250.754881	8991.059312	27.568794
251.026793	8998.603790	27.573812
251.211864	9013.896792	27.578829
251.476763	9019.623856	27.583847
251.763993	9032.930910	27.588864
252.266474	9036.894032	27.593882
252.673032	9046.858042	27.598900
252.543737	9050.477526	27.603917
252.730613	9061.306076	27.608935
253.251723	9081.115216	27.613952
253.388513	9089.558458	27.618970
253.421056	9097.092885	27.623988
253.749395	9120.045037	27.629005
254.013153	9121.636429	27.634023
254.044113	9139.832860	27.639040
254.591652	9151.754521	27.644058
255.071212	9155.967496	27.649076
255.253763	9170.740087	27.654093
255.542558	9179.645909	27.659111
255.691288	9193.116715	27.664128
255.929157	9200.458202	27.669146
256.049186	9206.027920	27.674164
256.076696	9223.842952	27.679181
256.649613	9234.482058	27.684199
256.595786	9257.168689	27.689216
257.116915	9259.405132	27.694234
257.766212	9273.808364	27.699252
257.626731	9280.024686	27.704269
258.171379	9291.754300	27.709287
258.348070	9302.837153	27.714304
258.606760	9311.580394	27.719322
258.879193	9324.741574	27.724340
259.022071	9327.867258	27.729357
259.546515	9343.612848	27.734375
259.950698	9350.006600	27.739392
260.106552	9359.728820	27.744410
260.243160	9364.263599	27.749428
260.366263	9386.171427	27.754445
260.902556	9370.946176	27.759463
260.976638	9393.259453	27.764480
261.219578	9400.748619	27.769498
261.484316	9404.685690	27.774516
261.640145	9419.813091	27.779533
262.042199	9422.121766	27.784551
262.365244	9427.426310	27.789568
262.407740	9431.331685	27.794586
262.427299	9443.427295	27.799604
262.655858	9454.416919	27.804621
262.743704	9454.769682	27.809639
263.198551	9471.407081	27.814656
263.531812	9481.550071	27.819674
263.387664	9491.309595	27.824692
263.587577	9517.196353	27.829709
264.374900	9526.460425	27.834727
264.055408	9547.518596	27.839744
264.463914	9556.633283	27.844762
264.693550	9577.252385	27.849780
264.867731	9605.356496	27.854797
265.364269	9611.852779	27.859815
265.624368	9634.285775	27.864832
266.010263	9646.232922	27.869850
266.400398	9667.044986	27.874868
266.704237	9677.587321	27.879885
266.945010	9690.497953	27.884903
267.140284	9693.337703	27.889920
267.483428	9717.775360	27.894938
267.694296	9726.043181	27.899956
267.551770	9749.255698	27.904973
268.587518	9751.626778	27.909991
268.644213	9764.825017	27.915008
269.078053	9778.965403	27.920026
269.329636	9788.461408	27.925044
269.689769	9809.764524	27.930061
269.914608	9808.511012	27.935079
270.249309	9833.357425	27.940096
270.592579	9833.357859	27.945114
270.760291	9848.502703	27.950132
270.786405	9862.905541	27.955149
271.283062	9864.912231	27.960167
271.630704	9880.796309	27.965184
271.374663	9881.354170	27.970202
272.334808	9897.929071	27.975220
272.201722	9914.244795	27.980237
272.547749	9919.230173	27.985255
272.529917	9934.160862	27.990272
272.719884	9950.195840	27.995290
273.171465	9966.988900	28.000308
273.318665	9981.833945	28.005325
273.548889	9986.951033	28.010343
273.936429	10004.634987	28.015360
274.671133	10033.779641	28.020378
274.813693	10042.920186	28.025396
274.895807	10058.817341	28.030413
275.206327	10069.513567	28.035431
275.568486	10080.362784	28.040448
275.560444	10105.907016	28.045466
276.168932	10112.758611	28.050484
276.263084	10129.421184	28.055501
276.533019	10134.140620	28.060519
276.916093	10149.845760	28.065536
277.071963	10168.986740	28.070554
277.140205	10183.721103	28.075572
277.679937	10206.464877	28.080589
278.048242	10207.386517	28.085607
277.870893	10225.067064	28.090624
278.131131	10241.473392	28.095642
278.821350	10250.197253	28.100660
278.802366	10267.859500	28.105677
279.518038	10289.281468	28.110695
279.880768	10296.007210	28.115712
280.056184	10312.464695	28.120730
280.511013	10314.872618	28.125748
280.264888	10331.979862	28.130765
280.295876	10346.060262	28.135783
280.647675	10353.021372	28.140800
280.777762	10375.339737	28.145818
281.614861	10392.477307	28.150836
281.490457	10410.474996	28.155853
281.736158	10417.850478	28.160871
282.599896	10434.185122	28.165888
282.521571	10442.469869	28.170906
282.886131	10449.830017	28.175924
283.134404	10466.197360	28.180941
283.626032	10471.472801	28.185959
283.798452	10486.434302	28.190976
284.314414	10510.287237	28.195994
284.501799	10512.023252	28.201012
284.402893	10527.418546	28.206029
284.719670	10541.479860	28.211047
285.277295	10550.540248	28.216064
285.418162	10573.573902	28.221082
285.803255	10575.642245	28.226100
285.776490	10592.803983	28.231117
286.272081	10604.943059	28.236135
286.701700	10625.036474	28.241152
286.786302	10642.177762	28.246170
287.641756	10651.141311	28.251188
287.578835	10676.799064	28.256205
287.995165	10678.717314	28.261223
288.291424	10695.708873	28.266240
288.512234	10711.124007	28.271258
289.138709	10722.346072	28.276276
289.029778	10737.228438	28.281293
289.467868	10749.600739	28.286311
289.699180	10754.935733	28.291328
289.638337	10769.798008	28.296346
290.565386	10770.942119	28.301364
290.253909	10788.306234	28.306381
290.529904	10804.072801	28.311399
291.236474	10817.019051	28.316416
291.319470	10835.022749	28.321434
291.872019	10852.558680	28.326452
292.302964	10861.244259	28.331469
292.286306	10872.111869	28.336487
292.651761	10872.579314	28.341504
293.005181	10889.192728	28.346522
293.555897	10902.482206	28.351540
293.691778	10907.017475	28.356557
293.958152	10918.478855	28.361575
294.293612	10932.041834	28.366592
294.361443	10951.680417	28.371610
295.288478	10953.326580	28.376628
295.131377	10961.961672	28.381645
295.255874	10977.704610	28.386663
295.580524	10992.118677	28.391680
295.714790	11007.168631	28.396698
296.085218	11013.978687	28.401716
296.501357	11034.093588	28.406733
296.535376	11043.617791	28.411751
296.614522	11059.045794	28.416768
296.990713	11086.887037	28.421786
297.365728	11092.022936	28.426804
297.827780	11108.979588	28.431821
298.358310	11110.412794	28.436839
298.631806	11127.345141	28.441856
298.558730	11146.535399	28.446874
299.074556	11159.176888	28.451892
298.861259	11169.045937	28.456909
299.400705	11179.852408	28.461927
299.929714	11205.324005	28.466944
299.975054	11222.831894	28.471962
300.304821	11231.312373	28.476980
300.552618	11248.892965	28.481997
300.658819	11266.110400	28.487015
300.857503	11278.261408	28.492032
301.203382	11302.921747	28.497050
301.521469	11313.993258	28.502068
301.842679	11341.947639	28.507085
302.188308	11358.117471	28.512103
302.638866	11373.241621	28.517120
302.809163	11392.056383	28.522138
303.155932	11402.308834	28.527156
303.269981	11426.749667	28.532173
303.434767	11458.299767	28.537191
304.144926	11463.307810	28.542208
303.817140	11494.830459	28.547226
304.601170	11510.581680	28.552244
305.017893	11535.777555	28.557261
305.152031	11551.525790	28.562279
305.500624	11563.492608	28.567296
305.789970	11591.152352	28.572314
306.256277	11600.069591	28.577332
306.820107	11615.905705	28.582349
306.872446	11632.699273	28.587367
307.102950	11639.477664	28.592384
307.432413	11664.867281	28.597402
307.998805	11685.439444	28.602420
308.382280	11696.829392	28.607437
308.470272	11715.995156	28.612455
309.242339	11734.937608	28.617472
309.579646	11752.785764	28.622490
309.940703	11759.329156	28.627508
310.044508	11769.786989	28.632525
310.244706	11790.065784	28.637543
310.882455	11795.375691	28.642560
310.799109	11817.962670	28.647578
311.111435	11830.948901	28.652596
311.393263	11849.247854	28.657613
311.461712	11868.521018	28.662631
311.986663	11893.394235	28.667648
312.238952	11908.019204	28.672666
312.584169	11933.188855	28.677684
313.272028	11948.166009	28.682701
313.536401	11967.111954	28.687719
313.872117	11979.163141	28.692736
314.076207	12005.160060	28.697754
314.501904	12012.662876	28.702772
314.845331	12028.571545	28.707789
315.061634	12049.208085	28.712807
315.767174	12056.042135	28.717824
315.636315	12069.346985	28.722842
316.090521	12081.951328	28.727860
316.468691	12086.850186	28.732877
316.373763	12104.112334	28.737895
316.809547	12107.300246	28.742912
317.253310	12142.297286	28.747930
317.466573	12150.171101	28.752948
317.926677	12155.701388	28.757965
318.279428	12176.746269	28.762983
319.032343	12188.236884	28.768000
319.461647	12199.901038	28.773018
319.547759	12219.408638	28.778036
319.807452	12221.815617	28.783053
319.986688	12229.637925	28.788071
320.184275	12239.525666	28.793088
320.395197	12264.511419	28.798106
320.261965	12277.415757	28.803124
320.789511	12295.007459	28.808141
321.090723	12314.191161	28.813159
321.731924	12331.086297	28.818176
321.610773	12351.740971	28.823194
321.740545	12364.465484	28.828212
322.692477	12382.338546	28.833229
322.602414	12400.787508	28.838247
322.736455	12412.687225	28.843264
322.844010	12439.861814	28.848282
323.545597	12459.801183	28.853300
323.918592	12473.151025	28.858317
324.301817	12497.958693	28.863335
324.606753	12514.631622	28.868352
324.789978	12528.194197	28.873370
324.901355	12543.441570	28.878388
325.656775	12564.111580	28.883405
325.587420	12591.263405	28.888423
325.963508	12606.576981	28.893440
326.367869	12622.962961	28.898458
326.740694	12635.807705	28.903476
327.494117	12662.841013	28.908493
327.603277	12678.243570	28.913511
328.269475	12703.023242	28.918528
327.999979	12704.208513	28.923546
328.678384	12726.425367	28.928564
329.523545	12736.856737	28.933581
330.217729	12758.799604	28.938599
330.417054	12763.091771	28.943616
330.612154	12776.690570	28.948634
330.826524	12779.167833	28.953652
331.915003	12776.150260	28.958669
331.892320	12787.708311	28.963687
332.642952	12780.095082	28.968704
332.799056	12795.651474	28.973722
332.714974	12810.054786	28.978740
333.153701	12820.284225	28.983757
332.991308	12830.231478	28.988775
333.612885	12832.048530	28.993792
333.689596	12849.382531	28.998810
333.786723	12874.077346	29.003828
334.621359	12885.470408	29.008845
334.542320	12896.427845	29.013863
334.917064	12915.749130	29.018880
334.661866	12936.299001	29.023898
335.180100	12955.244313	29.028916
335.448882	12970.360160	29.033933
335.602733	12994.923147	29.038951
336.071042	13010.049015	29.043968
336.416827	13044.453528	29.048986
336.637131	13067.421036	29.054004
337.217698	13088.734623	29.059021
336.881109	13113.977264	29.064039
337.544731	13130.266483	29.069056
337.864077	13166.143729	29.074074
338.345402	13188.237076	29.079092
338.707255	13216.219497	29.084109
338.987038	13240.832671	29.089127
339.558156	13252.355403	29.094144
339.973555	13282.066407	29.099162
339.929678	13310.093185	29.104180
341.033760	13326.525578	29.109197
340.808665	13351.331181	29.114215
341.506474	13362.679521	29.119232
342.090093	13387.558213	29.124250
342.482328	13397.634153	29.129268
342.788209	13403.049873	29.134285
343.004844	13425.658390	29.139303
343.324221	13441.786735	29.144320
343.657277	13456.264545	29.149338
344.019181	13482.665249	29.154356
344.267260	13483.302620	29.159373
344.207352	13506.330076	29.164391
344.576925	13529.821224	29.169408
344.747767	13546.980156	29.174426
345.505703	13563.204540	29.179444
345.904925	13571.315265	29.184461
346.055770	13598.266885	29.189479
346.685591	13621.597631	29.194496
347.005329	13622.236482	29.199514
347.043899	13651.169885	29.204532
347.549790	13668.519925	29.209549
347.798386	13695.339623	29.214567
348.159070	13708.130146	29.219584
348.677858	13718.972881	29.224602
349.018031	13740.011994	29.229620
349.439911	13758.518371	29.234637
349.777425	13772.670461	29.239655
350.179816	13788.385120	29.244672
350.178597	13804.355262	29.249690
350.631893	13829.655887	29.254708
350.850450	13846.725555	29.259725
351.085052	13876.048790	29.264743
351.566515	13878.225664	29.269760
351.855336	13901.938272	29.274778
352.157415	13936.840698	29.279796
353.040825	13941.891918	29.284813
353.399825	13975.636052	29.289831
354.242602	13985.487423	29.294848
354.334071	13996.456846	29.299866
354.700980	14012.676176	29.304884
355.251114	14023.631052	29.309901
355.618532	14043.118847	29.314919
355.767429	14054.916231	29.319936
356.269872	14068.284948	29.324954
356.004571	14085.635430	29.329972
357.030544	14103.157542	29.334989
356.805695	14117.580605	29.340007
357.020653	14136.078512	29.345024
357.460506	14156.379386	29.350042
357.780086	14186.289892	29.355060
358.383950	14203.985186	29.360077
358.811786	14232.688339	29.365095
359.099420	14251.086619	29.370112
359.141820	14268.509369	29.375130
359.424513	14290.578085	29.380148
359.869952	14299.503016	29.385165
360.384334	14325.647462	29.390183
360.622666	14342.395537	29.395200
361.123270	14364.822011	29.400218
361.319501	14386.291639	29.405236
361.881794	14404.887320	29.410253
362.165136	14444.303293	29.415271
362.457758	14461.949383	29.420288
363.110786	14477.751917	29.425306
363.379368	14502.346368	29.430324
364.025305	14514.770906	29.435341
364.411855	14528.164307	29.440359
364.970524	14537.314894	29.445376
365.364017	14544.969009	29.450394
365.579969	14560.855448	29.455412
366.049931	14579.250926	29.460429
366.693096	14591.666472	29.465447
366.944277	14611.438226	29.470464
367.552326	14612.682794	29.475482
367.173695	14632.568411	29.480500
367.650900	14642.912857	29.485517
368.035461	14667.798960	29.490535
368.196779	14680.911724	29.495552
368.700473	14685.201158	29.500570
368.725680	14710.449597	29.505588
368.937144	14725.679988	29.510605
368.927252	14743.572397	29.515623
369.707742	14753.228592	29.520640
370.265441	14778.492123	29.525658
370.476801	14799.931439	29.530676
370.797347	14816.171308	29.535693
371.154975	14845.660058	29.540711
371.439630	14861.056017	29.545728
371.956855	14888.861971	29.550746
372.189689	14903.994434	29.555764
372.495542	14926.701385	29.560781
372.660809	14950.349268	29.565799
373.397437	14977.274812	29.570816
374.110448	14992.736833	29.575834
374.127931	15026.794970	29.580852
374.593601	15041.818657	29.585869
375.271579	15068.222890	29.590887
375.414551	15075.404600	29.595904
375.914223	15108.345621	29.600922
376.037818	15145.498246	29.605940
376.524695	15149.184035	29.610957
377.018094	15164.680385	29.615975
377.238193	15193.297321	29.620992
377.644018	15213.402499	29.626010
378.159678	15242.229306	29.631028
378.132387	15263.425220	29.636045
378.331970	15279.513773	29.641063
378.781640	15310.489056	29.646080
379.552146	15334.624300	29.651098
379.762849	15358.470899	29.656116
380.379986	15381.471016	29.661133
380.559803	15410.956741	29.666151
380.588310	15434.538086	29.671168
381.555866	15456.245717	29.676186
382.097293	15482.198050	29.681204
382.436252	15503.646717	29.686221
383.159043	15514.828236	29.691239
383.515130	15538.447141	29.696256
384.024432	15545.957302	29.701274
384.131026	15573.202853	29.706292
384.351936	15589.929471	29.711309
384.869015	15609.742980	29.716327
385.299050	15639.954400	29.721344
385.761494	15647.771931	29.726362
385.726535	15672.730975	29.731380
386.014769	15688.297592	29.736397
386.529021	15715.489354	29.741415
386.584475	15742.171460	29.746432
386.868350	15764.102736	29.751450
387.533043	15780.526720	29.756468
387.957199	15824.007277	29.761485
388.673430	15839.567393	29.766503
389.284146	15859.824536	29.771520
389.540066	15875.108931	29.776538
389.774719	15902.502403	29.781556
390.163836	15916.010081	29.786573
390.847629	15935.182105	29.791591
391.062476	15955.908401	29.796608
391.518114	15967.725540	29.801626
391.684425	15995.319283	29.806644
392.551908	16026.161198	29.811661
392.499369	16036.996300	29.816679
392.730020	16060.616428	29.821696
393.584280	16076.559515	29.826714
393.651799	16106.114327	29.831732
393.527843	16126.937771	29.836749
394.203626	16137.940634	29.841767
394.346154	16159.111101	29.846784
394.716232	16167.862303	29.851802
395.168171	16203.591985	29.856820
395.743883	16228.548274	29.861837
396.231047	16252.330840	29.866855
396.250124	16285.348711	29.871872
396.948330	16302.952313	29.876890
397.286920	16329.477456	29.881908
397.440124	16351.584509	29.886925
398.336012	16368.952103	29.891943
398.601602	16388.919274	29.896960
399.160183	16405.088695	29.901978
399.212935	16436.326574	29.906996
399.437479	16457.393008	29.912013
400.079968	16478.887108	29.917031
400.307659	16512.087662	29.922048
401.088103	16534.094117	29.927066
402.128813	16557.127619	29.932084
402.428194	16568.663091	29.937101
402.757836	16582.035213	29.942119
402.933753	16608.437622	29.947136
403.502577	16622.360000	29.952154
403.879288	16644.236772	29.957172
403.842490	16665.369388	29.962189
404.338854	16680.007418	29.967207
404.713422	16711.745209	29.972224
405.443921	16729.751616	29.977242
405.717853	16759.411111	29.982260
405.819580	16785.916908	29.987277
406.430474	16806.787765	29.992295
406.539715	16829.622338	29.997312
406.803560	16848.175273	30.002330
407.411238	16881.055156	30.007348
407.816023	16913.442377	30.012365
408.573801	16933.485097	30.017383
408.406438	16962.461891	30.022400
409.242022	16983.967557	30.027418
409.400068	17019.125451	30.032436
409.767309	17045.609221	30.037453
410.548425	17066.564407	30.042471
410.955493	17097.827161	30.047488
411.250601	17116.009102	30.052506
411.708593	17141.430255	30.057524
412.114963	17168.950409	30.062541
412.517391	17189.573030	30.067559
412.865546	17224.666958	30.072576
413.095939	17252.284115	30.077594
413.798258	17278.712882	30.082612
414.031716	17302.343576	30.087629
414.642423	17325.356508	30.092647
415.266465	17351.917587	30.097664
415.567488	17367.069808	30.102682
416.034868	17391.949720	30.107700
416.632773	17413.578151	30.112717
417.419636	17421.165867	30.117735
417.913264	17437.488407	30.122752
418.677886	17449.495251	30.127770
418.952467	17460.754009	30.132788
419.070405	17486.140118	30.137805
419.588301	17491.868284	30.142823
420.160520	17505.313834	30.147840
420.452738	17519.447331	30.152858
420.897278	17540.957646	30.157876
420.395479	17547.245714	30.162893
421.144561	17570.850160	30.167911
420.984385	17589.719349	30.172928
421.559413	17621.771718	30.177946
421.859933	17639.021530	30.182964
422.156402	17671.445840	30.187981
422.598384	17689.722325	30.192999
423.183923	17717.907102	30.198016
423.497117	17742.173434	30.203034
423.770839	17764.380215	30.208052
424.134706	17795.739268	30.213069
424.804396	17815.502872	30.218087
424.770345	17843.777974	30.223104
425.500856	17872.843772	30.228122
426.044736	17903.145265	30.233140
426.628030	17924.912366	30.238157
427.107048	17941.142849	30.243175
427.922278	17971.376935	30.248192
428.338837	17990.592620	30.253210
428.850695	18010.159891	30.258228
429.310788	18030.392239	30.263245
429.835540	18040.892219	30.268263
430.047844	18068.295413	30.273280
430.416693	18080.500089	30.278298
430.678633	18105.930925	30.283316
431.125540	18134.112623	30.288333
431.694380	18155.888553	30.293351
431.988151	18187.954062	30.298368
432.327920	18204.320158	30.303386
432.766421	18227.247265	30.308404
433.095062	18266.086001	30.313421
433.663954	18286.270093	30.318439
434.171171	18313.431883	30.323456
434.622938	18341.341479	30.328474
435.280550	18362.402591	30.333492
435.445051	18391.342495	30.338509
436.413722	18418.236753	30.343527
436.523928	18435.535857	30.348544
436.891821	18463.180719	30.353562
437.301008	18479.176146	30.358580
437.664308	18499.935768	30.363597
438.583878	18525.612235	30.368615
438.566273	18558.497562	30.373632
439.000218	18573.851149	30.378650
439.349463	18608.366214	30.383668
439.649654	18641.334875	30.388685
440.048277	18655.752719	30.393703
440.698728	18693.316618	30.398720
440.709222	18722.514740	30.403738
441.223763	18748.570434	30.408756
441.335366	18788.157886	30.413773
442.310137	18810.414666	30.418791
442.777715	18841.032749	30.423808
443.122607	18879.554306	30.428826
444.042832	18897.757481	30.433844
444.263084	18913.372038	30.438861
444.822793	18943.198876	30.443879
445.572943	18969.578291	30.448896
445.737781	18989.074225	30.453914
446.857043	19013.880011	30.458932
446.903883	19038.113623	30.463949
447.476504	19052.207747	30.468967
447.803007	19072.013430	30.473984
448.012369	19088.198410	30.479002
448.512389	19114.402163	30.484020
448.672750	19148.859147	30.489037
449.129607	19170.729465	30.494055
449.634731	19210.736655	30.499072
449.721176	19232.279330	30.504090
450.499684	19260.493172	30.509108
450.651635	19299.127728	30.514125
451.237087	19321.660508	30.519143
451.589451	19347.198931	30.524160
452.076872	19366.897732	30.529178
452.889618	19388.599172	30.534196
452.683383	19418.729197	30.539213
453.556759	19436.630604	30.544231
453.910936	19463.268186	30.549248
454.227195	19495.010146	30.554266
454.936384	19521.295604	30.559284
455.145498	19551.493846	30.564301
455.573339	19581.702308	30.569319
455.901441	19605.197880	30.574336
456.384701	19635.385162	30.579354
457.034741	19661.882188	30.584372
457.396077	19697.363931	30.589389
457.829988	19733.017658	30.594407
458.594029	19766.225586	30.599424
458.759975	19789.531818	30.604442
459.508044	19817.182600	30.609460
459.813111	19844.321142	30.614477
460.849805	19870.669808	30.619495
461.269299	19895.092867	30.624512
461.447323	19927.684698	30.629530
462.179643	19935.196612	30.634548
462.218586	19970.305741	30.639565
462.940820	19996.065422	30.644583
463.384364	20024.698961	30.649600
463.831470	20062.284525	30.654618
464.296246	20083.826103	30.659636
464.856981	20111.721278	30.664653
465.142721	20138.092445	30.669671
465.863477	20173.904497	30.674688
465.831266	20195.062354	30.679706
466.976662	20217.780675	30.684724
467.074052	20244.029675	30.689741
467.415450	20278.270929	30.694759
468.184902	20302.665290	30.699776
468.491957	20332.502000	30.704794
468.991524	20348.573350	30.709812
469.251982	20386.081187	30.714829
470.343539	20413.413983	30.719847
471.005620	20427.286682	30.724864
471.396154	20452.011896	30.729882
472.097088	20465.354174	30.734900
472.392583	20491.528439	30.739917
472.907574	20516.215404	30.744935
473.279310	20536.103988	30.749952
473.221336	20565.486114	30.754970
473.703765	20590.993281	30.759988
474.138118	20619.837621	30.765005
474.633281	20649.891938	30.770023
475.116970	20677.389236	30.775040
475.564925	20710.546890	30.780058
476.159649	20728.625551	30.785076
476.809234	20768.600810	30.790093
477.106594	20792.134186	30.795111
478.039731	20816.137252	30.800128
478.035309	20843.451726	30.805146
478.524374	20863.214966	30.810164
478.961572	20904.613573	30.815181
479.183430	20926.528763	30.820199
479.718498	20952.900122	30.825216
479.962572	20991.479452	30.830234
480.633597	21025.045188	30.835252
480.971865	21061.095322	30.840269
481.322660	21092.885046	30.845287
481.760165	21133.039385	30.850304
481.923594	21164.637253	30.855322
482.762652	21198.278220	30.860340
483.418714	21229.850048	30.865357
483.939248	21261.089199	30.870375
484.794829	21276.707832	30.875392
484.856860	21307.456103	30.880410
485.648320	21333.636419	30.885428
486.019560	21359.067119	30.890445
486.656850	21380.400035	30.895463
487.215055	21406.629399	30.900480
487.596007	21434.510219	30.905498
488.075780	21457.472613	30.910516
488.432474	21489.925494	30.915533
488.819526	21520.617181	30.920551
489.486189	21539.386736	30.925568
490.197012	21580.889494	30.930586
490.698250	21603.810808	30.935604
491.033160	21632.463608	30.940621
491.374491	21654.923354	30.945639
492.033671	21678.174000	30.950656
492.552882	21727.971464	30.955674
493.064329	21753.425076	30.960692
493.169048	21788.198653	30.965709
493.552306	21810.633094	30.970727
494.117126	21835.250778	30.975744
494.629223	21881.922069	30.980762
495.486353	21907.189376	30.985780
496.085617	21938.606903	30.990797
496.557511	21978.012023	30.995815
497.015938	21995.904559	31.000832
497.440916	22029.244935	31.005850
498.084206	22062.665117	31.010868
498.196275	22093.463691	31.015885
498.914815	22128.818400	31.020903
499.421965	22148.535889	31.025920
500.197292	22180.520343	31.030938
500.409216	22210.134606	31.035956
500.953760	22240.828171	31.040973
501.351261	22284.118819	31.045991
501.489526	22310.553773	31.051008
502.033590	22344.786033	31.056026
502.915681	22379.584961	31.061044
503.495192	22410.677743	31.066061
503.597896	22458.071275	31.071079
504.573507	22484.003300	31.076096
505.112326	22515.879787	31.081114
504.955799	22558.404255	31.086132
505.874129	22592.787198	31.091149
506.817302	22619.514297	31.096167
506.876055	22656.621867	31.101184
507.338475	22699.808535	31.106202
508.109133	22728.761582	31.111220
508.915129	22752.862636	31.116237
509.270272	22783.567574	31.121255
510.020967	22811.083156	31.126272
510.082127	22844.235112	31.131290
510.788925	22864.143395	31.136308
511.180001	22892.669222	31.141325
511.654043	22928.499428	31.146343
512.492125	22956.210131	31.151360
512.954682	22993.362889	31.156378
513.669820	23020.840067	31.161396
514.097084	23053.328763	31.166413
513.905197	23088.732140	31.171431
514.438165	23118.000792	31.176448
514.882767	23156.982822	31.181466
515.465113	23187.412895	31.186484
516.259944	23222.972530	31.191501
516.535451	23248.527990	31.196519
517.230920	23278.921636	31.201536
517.166518	23324.782464	31.206554
518.305241	23340.023755	31.211572
519.104090	23356.423796	31.216589
519.823936	23377.746023	31.221607
520.453169	23404.270297	31.226624
521.257979	23421.844803	31.231642
521.394091	23446.398536	31.236660
522.112381	23461.844393	31.241677
522.414379	23481.392941	31.246695
523.095404	23496.117935	31.251712
523.545084	23526.487034	31.256730
523.820144	23539.878748	31.261748
523.894943	23580.928644	31.266765
524.533534	23606.345894	31.271783
525.187529	23633.763931	31.276800
525.405316	23668.864437	31.281818
526.251151	23701.345904	31.286836
526.469719	23730.386364	31.291853
526.831033	23765.540526	31.296871
527.220960	23796.216339	31.301888
527.906536	23831.035775	31.306906
528.464112	23871.846816	31.311924
529.080842	23904.351643	31.316941
529.596105	23942.098292	31.321959
530.116832	23979.641948	31.326976
530.434055	24026.443415	31.331994
530.879539	24056.877169	31.337012
531.612631	24093.395860	31.342029
532.238671	24134.746555	31.347047
533.604209	24173.631445	31.352064
533.988519	24209.136689	31.357082
533.989438	24224.271427	31.362100
534.876597	24260.810675	31.367117
535.342563	24289.111993	31.372135
535.756876	24323.374186	31.377152
536.691062	24354.433759	31.382170
537.029097	24395.659209	31.387188
537.771858	24404.738420	31.392205
537.997156	24440.287788	31.397223
538.493964	24470.821613	31.402240
539.234025	24511.472848	31.407258
539.721940	24545.218414	31.412276
540.290952	24569.447043	31.417293
540.779097	24602.737674	31.422311
541.343972	24635.890027	31.427328
542.051222	24669.064507	31.432346
542.644028	24704.260119	31.437364
543.554525	24722.508143	31.442381
543.539916	24765.912588	31.447399
543.887013	24786.896231	31.452416
544.932308	24807.253008	31.457434
545.157928	24847.106606	31.462452
545.769593	24880.416388	31.467469
546.128171	24919.187757	31.472487
546.529002	24941.218555	31.477504
547.393580	24982.078866	31.482522
547.665987	25024.219520	31.487540
548.353704	25060.481624	31.492557
548.900765	25094.996215	31.497575
549.907850	25125.780219	31.502592
550.247021	25152.345660	31.507610
550.399478	25183.926355	31.512628
551.108967	25215.906992	31.517645
551.687121	25246.581009	31.522663
552.029909	25283.718764	31.527680
552.582831	25327.977696	31.532698
553.315440	25353.192949	31.537716
553.813153	25392.291153	31.542733
554.570811	25418.886593	31.547751
554.876071	25437.159978	31.552768
555.234015	25472.090158	31.557786
555.696486	25510.486276	31.562804
556.348922	25541.882265	31.567821
556.485753	25572.985707	31.572839
557.124962	25613.041869	31.577856
557.903219	25645.214717	31.582874
558.615998	25683.325729	31.587892
559.141530	25716.138409	31.592909
559.355980	25740.840758	31.597927
559.981542	25776.898963	31.602944
560.829625	25821.707093	31.607962
560.735556	25862.332931	31.612980
561.905061	25900.809320	31.617997
562.050281	25947.313421	31.623015
562.598582	25980.287304	31.628032
563.378654	26017.882887	31.633050
563.715042	26069.792581	31.638068
564.215454	26108.480968	31.643085
565.142459	26149.251780	31.648103
565.907230	26182.084857	31.653120
566.557622	26223.644630	31.658138
567.257891	26266.467030	31.663156
567.443909	26303.871231	31.668173
567.945707	26345.814626	31.673191
568.173509	26386.081732	31.678208
569.193277	26413.149603	31.683226
569.734089	26465.862728	31.688244
570.268335	26498.251888	31.693261
571.027669	26535.352387	31.698279
571.758082	26585.476705	31.703296
572.507017	26615.077100	31.708314
573.230111	26646.824056	31.713332
573.398259	26685.236632	31.718349
574.207058	26728.738325	31.723367
574.647542	26754.582261	31.728384
575.587769	26802.253864	31.733402
576.119718	26833.266139	31.738420
576.631734	26857.177760	31.743437
577.546708	26888.244254	31.748455
578.001848	26918.465962	31.753472
578.796265	26940.153273	31.758490
579.362751	26979.534580	31.763508
580.203556	27007.117761	31.768525
580.830186	27030.025800	31.773543
581.509138	27055.535950	31.778560
582.125520	27076.429501	31.783578
582.872057	27109.620858	31.788596
583.253488	27126.638841	31.793613
583.756755	27163.369545	31.798631
584.034223	27179.626371	31.803648
584.828716	27214.295684	31.808666
585.322214	27244.619352	31.813684
585.678496	27273.340126	31.818701
585.735041	27303.769827	31.823719
586.300297	27336.003817	31.828736
586.851373	27366.356626	31.833754
587.146324	27420.798027	31.838772
588.016852	27458.281090	31.843789
588.445808	27505.743211	31.848807
589.156437	27542.594009	31.853824
589.628765	27582.894953	31.858842
590.129883	27633.822326	31.863860
590.627098	27664.462061	31.868877
591.125165	27716.780596	31.873895
591.635565	27757.948173	31.878912
592.730708	27789.379870	31.883930
593.131713	27823.700656	31.888948
593.549526	27862.373655	31.893965
593.874113	27904.107690	31.898983
594.576389	27935.398519	31.904000
595.260974	27973.120054	31.909018
595.969820	28017.878888	31.914036
596.211002	28045.613716	31.919053
597.173166	28102.177884	31.924071
597.844410	28132.494170	31.929088
598.431236	28177.430362	31.934106
598.579657	28228.964016	31.939124
599.601049	28257.614243	31.944141
600.198721	28303.389658	31.949159
600.705533	28345.134153	31.954176
601.394227	28383.475226	31.959194
601.436032	28432.674735	31.964212
602.293074	28468.733307	31.969229
603.060351	28510.797869	31.974247
603.572526	28570.574740	31.979264
604.528719	28611.485025	31.984282
605.146124	28650.646743	31.989300
606.160400	28691.883144	31.994317
606.489146	28726.418962	31.999335
606.817079	28764.083712	32.004352
607.957685	28803.650969	32.009370
608.509368	28843.644982	32.014388
609.152275	28883.953551	32.019405
609.584269	28915.787302	32.024423
610.109575	28952.340825	32.029440
611.291856	28986.681002	32.034458
611.648856	29028.652482	32.039476
612.511777	29064.414117	32.044493
612.844626	29098.703415	32.049511
613.805286	29145.574598	32.054528
614.638295	29175.753480	32.059546
614.969833	29216.534672	32.064564
615.895038	29244.025586	32.069581
616.639816	29282.290089	32.074599
617.041057	29307.448087	32.079616
617.291275	29339.904958	32.084634
618.189737	29375.642642	32.089652
618.821886	29416.510175	32.094669
619.316223	29443.189826	32.099687
619.666841	29487.445090	32.104704
620.487583	29510.888271	32.109722
620.825686	29563.015209	32.114740
621.561226	29605.207064	32.119757
622.364568	29637.723682	32.124775
622.751930	29675.861252	32.129792
623.115053	29728.800123	32.134810
623.779242	29766.332199	32.139828
624.675109	29798.954768	32.144845
625.452054	29838.169777	32.149863
626.018880	29881.658992	32.154880
626.690815	29920.239437	32.159898
627.182569	29957.918807	32.164916
627.785149	29996.415376	32.169933
628.807375	30035.510404	32.174951
628.643746	30072.754717	32.179968
629.588319	30112.272851	32.184986
629.898167	30155.511880	32.190004
630.744604	30196.948115	32.195021
631.340563	30243.132690	32.200039
631.907549	30294.492597	32.205056
632.601080	30328.323246	32.210074
632.885495	30379.746318	32.215092
633.819955	30418.078230	32.220109
634.755977	30456.087588	32.225127
635.116649	30497.669584	32.230144
635.525762	30531.190853	32.235162
635.975995	30570.862680	32.240180
636.710464	30601.583667	32.245197
637.653234	30645.218254	32.250215
637.941410	30687.203836	32.255232
638.865929	30718.009195	32.260250
639.456199	30767.255341	32.265268
639.898111	30815.437431	32.270285
640.742240	30847.848475	32.275303
641.035655	30896.957824	32.280320
641.806560	30934.658738	32.285338
642.503029	30980.064431	32.290356
643.496502	31020.183551	32.295373
643.959389	31062.907588	32.300391
644.207703	31112.119290	32.305408
644.947733	31160.104060	32.310426
645.764385	31210.611917	32.315444
646.271513	31252.400205	32.320461
647.096807	31295.934348	32.325479
647.902623	31343.675409	32.330496
648.729613	31382.114346	32.335514
649.371434	31424.014764	32.340532
650.252887	31462.533874	32.345549
651.242700	31491.174582	32.350567
651.776681	31529.065181	32.355584
652.424123	31573.044817	32.360602
652.963200	31611.048561	32.365620
653.880806	31643.809747	32.370637
654.751614	31678.771864	32.375655
655.151040	31720.166959	32.380672
655.723862	31756.351415	32.385690
656.156492	31794.852510	32.390708
657.010061	31835.134068	32.395725
657.602012	31870.835301	32.400743
658.074675	31916.821553	32.405760
658.861030	31949.078956	32.410778
659.014426	31992.915133	32.415796
659.555996	32048.714862	32.420813
660.615918	32080.563224	32.425831
661.197435	32131.147860	32.430848
661.780355	32170.346933	32.435866
662.741898	32225.607628	32.440884
663.463028	32265.189957	32.445901
664.068228	32303.614557	32.450919
664.341966	32357.395906	32.455936
665.275717	32390.162081	32.460954
665.985564	32431.731533	32.465972
666.558794	32479.182681	32.470989
667.265708	32520.190123	32.476007
667.537882	32584.833247	32.481024
668.491294	32620.365704	32.486042
668.985750	32676.035368	32.491060
669.682030	32723.309869	32.496077
670.465791	32762.997190	32.501095
670.849096	32818.678215	32.506112
671.685858	32849.791221	32.511130
672.484247	32912.166047	32.516148
673.085674	32953.475251	32.521165
673.737356	33002.856227	32.526183
674.462843	33059.129469	32.531200
675.300160	33106.332307	32.536218
675.932358	33148.775073	32.541236
676.550638	33201.891724	32.546253
677.136700	33242.198685	32.551271
677.622953	33292.434289	32.556288
678.576377	33328.043817	32.561306
679.196415	33369.509000	32.566324
679.895028	33417.770959	32.571341
681.212875	33447.292656	32.576359
682.162923	33484.540410	32.581376
682.553756	33514.484686	32.586394
683.098128	33549.368001	32.591412
683.406058	33591.476494	32.596429
684.491283	33605.172294	32.601447
684.703329	33657.936079	32.606464
685.634815	33691.140886	32.611482
686.152686	33736.125202	32.616500
686.797667	33779.686293	32.621517
688.095477	33803.881973	32.626535
688.658352	33850.718269	32.631552
689.429660	33884.137985	32.636570
690.320071	33915.844844	32.641588
690.492784	33955.439886	32.646605
691.137516	33993.520039	32.651623
691.611276	34037.911252	32.656640
692.283098	34079.331846	32.661658
692.877798	34125.209130	32.666676
693.449050	34166.051251	32.671693
694.209746	34215.582498	32.676711
694.965056	34274.174671	32.681728
695.553369	34320.394784	32.686746
696.599963	34374.149516	32.691764
696.510327	34423.402669	32.696781
697.414800	34466.539121	32.701799
698.210110	34523.703213	32.706816
699.155096	34581.545956	32.711834
699.962406	34633.182637	32.716852
700.247798	34692.095703	32.721869
701.290718	34738.656928	32.726887
702.126275	34780.603474	32.731904
703.265613	34813.335125	32.736922
704.110385	34867.773759	32.741940
704.494803	34908.064730	32.746957
705.735569	34944.858855	32.751975
706.537232	34984.237793	32.756992
707.207469	35024.642558	32.762010
708.113994	35071.074009	32.767028
708.534370	35105.568241	32.772045
709.154872	35138.147228	32.777063
709.959463	35176.849548	32.782080
710.160684	35233.298748	32.787098
710.837730	35272.558525	32.792116
711.828169	35321.177756	32.797133
712.202913	35365.397500	32.802151
713.169388	35415.171411	32.807168
713.809402	35451.680579	32.812186
714.505197	35504.120771	32.817204
715.103515	35548.483130	32.822221
715.943094	35593.237973	32.827239
716.593744	35632.534142	32.832256
717.421746	35691.871350	32.837274
717.828032	35735.271313	32.842292
718.473884	35785.032779	32.847309
719.095780	35839.786817	32.852327
720.099560	35885.420885	32.857344
720.768905	35931.568683	32.862362
721.626103	35981.487396	32.867380
722.266956	36034.835305	32.872397
722.878399	36070.597562	32.877415
723.541943	36124.074945	32.882432
724.351414	36176.322063	32.887450
725.429356	36218.353868	32.892468
725.717588	36275.532084	32.897485
726.774383	36318.661256	32.902503
727.404306	36359.991680	32.907520
727.986797	36414.626876	32.912538
728.828436	36449.367545	32.917556
728.927844	36497.420005	32.922573
729.444786	36536.776602	32.927591
730.076171	36584.215308	32.932608
731.015517	36644.214413	32.937626
731.875943	36698.073592	32.942644
732.160011	36744.283131	32.947661
733.231076	36799.298523	32.952679
733.701099	36849.235284	32.957696
734.709742	36901.611257	32.962714
735.354709	36949.396436	32.967732
736.179261	37011.937396	32.972749
737.189824	37063.934079	32.977767
737.903672	37122.515296	32.982784
738.280048	37170.873934	32.987802
739.256917	37218.159098	32.992820
739.789571	37284.103945	32.997837
740.483537	37326.229331	33.002855
741.287723	37392.625460	33.007872
741.931866	37453.267187	33.012890
743.524034	37502.556543	33.017908
743.888650	37561.579053	33.022925
744.663173	37609.623769	33.027943
745.188351	37660.932336	33.032960
746.071345	37717.440075	33.037978
746.931465	37776.341778	33.042996
747.561566	37824.320930	33.048013
748.315554	37882.126520	33.053031
748.887246	37952.911116	33.058048
749.551646	38007.436460	33.063066
750.785594	38064.465919	33.068084
751.546746	38124.711922	33.073101
752.232906	38186.398888	33.078119
752.708376	38243.142188	33.083136
753.388629	38301.624360	33.088154
754.493828	38360.742459	33.093172
755.151438	38424.597223	33.098189
755.556669	38470.273088	33.103207
756.752886	38535.005527	33.108224
757.112267	38599.830488	33.113242
758.653446	38655.605872	33.118260
759.363250	38710.416821	33.123277
760.150774	38758.778272	33.128295
761.144194	38814.405361	33.133312
761.730974	38865.397353	33.138330
762.641779	38917.534215	33.143348
763.522238	38967.253923	33.148365
764.233740	39018.277452	33.153383
765.061195	39071.401525	33.158400
765.881412	39120.549174	33.163418
766.849052	39173.695944	33.168436
767.195438	39219.894788	33.173453
767.915751	39274.364048	33.178471
768.803890	39321.224991	33.183488
769.266731	39376.689494	33.188506
770.005687	39417.502933	33.193524
770.866097	39470.034735	33.198541
771.459801	39532.144677	33.203559
772.198095	39590.614988	33.208576
772.677871	39654.735063	33.213594
773.643587	39704.930144	33.218612
774.370169	39764.085737	33.223629
775.438569	39817.610494	33.228647
776.001507	39868.286039	33.233664
776.793682	39929.386000	33.238682
777.655385	39978.105430	33.243700
778.145599	40039.840846	33.248717
778.364835	40080.173596	33.253735
779.592529	40129.045087	33.258752
780.367053	40191.122446	33.263770
781.484348	40240.966319	33.268788
781.945632	40303.902253	33.273805
782.769574	40340.163454	33.278823
784.067544	40397.113229	33.283840
784.445591	40441.893131	33.288858
785.527768	40486.443355	33.293876
785.898577	40552.145125	33.298893
787.017837	40591.680999	33.303911
788.010757	40649.020431	33.308928
788.505064	40712.502617	33.313946
789.355718	40759.378830	33.318964
790.409421	40812.838765	33.323981
791.068238	40862.938842	33.328999
792.197067	40908.304831	33.334016
792.765477	40966.172858	33.339034
793.495992	41006.016651	33.344052
794.244309	41068.233405	33.349069
794.876874	41121.911441	33.354087
795.760378	41182.159561	33.359104
796.214289	41245.314392	33.364122
797.288168	41296.716931	33.369140
798.059158	41363.864070	33.374157
798.614231	41422.247664	33.379175
799.485500	41474.365207	33.384192
800.044624	41534.962047	33.389210
801.358461	41593.911032	33.394228
802.077793	41657.044708	33.399245
802.722341	41722.024334	33.404263
803.427754	41777.792399	33.409280
804.176041	41839.720422	33.414298
805.306717	41905.168833	33.419316
806.283657	41967.605543	33.424333
806.972393	42027.551104	33.429351
808.106789	42088.167443	33.434368
808.517284	42152.754701	33.439386
809.772180	42202.581642	33.444404
810.910411	42249.549108	33.449421
811.466320	42312.779684	33.454439
812.334296	42361.724831	33.459456
813.580517	42415.639401	33.464474
815.302049	42452.624559	33.469492
816.240971	42493.279817	33.474509
816.681500	42542.500626	33.479527
817.565272	42575.789895	33.484544
818.186130	42616.102753	33.489562
818.801533	42657.023720	33.494580
819.661129	42709.051144	33.499597
820.200222	42761.299355	33.504615
821.032194	42794.287101	33.509632
821.636329	42845.304684	33.514650
822.409435	42891.242480	33.519668
823.014755	42948.490154	33.524685
823.723598	43010.864039	33.529703
824.561712	43053.503084	33.534720
825.222396	43127.168518	33.539738
826.295196	43168.601132	33.544756
826.709335	43226.410586	33.549773
827.383184	43294.805803	33.554791
827.965550	43350.748813	33.559808
829.147717	43417.869850	33.564826
830.188538	43468.757647	33.569844
831.097941	43532.518602	33.574861
832.041743	43591.916386	33.579879
832.883302	43641.482026	33.584896
833.398979	43701.123852	33.589914
834.311148	43742.203040	33.594932
834.809033	43789.760511	33.599949
835.780117	43846.175578	33.604967
836.842007	43896.232481	33.609984
837.253878	43950.464120	33.615002
838.218864	44008.790765	33.620020
838.779471	44062.360675	33.625037
839.123418	44121.872234	33.630055
839.899353	44179.045932	33.635072
841.039880	44255.714511	33.640090
841.839421	44312.511686	33.645108
843.019182	44367.004326	33.650125
844.268786	44439.039069	33.655143
844.820467	44494.603897	33.660160
845.531638	44569.240374	33.665178
846.600182	44621.562368	33.670196
847.431394	44681.214637	33.675213
848.350836	44742.675057	33.680231
849.471144	44792.016439	33.685248
849.928241	44849.924644	33.690266
851.028322	44909.668507	33.695284
851.684535	44970.987094	33.700301
852.399424	45037.812569	33.705319
853.519556	45097.003493	33.710336
854.042979	45167.901180	33.715354
855.068332	45234.963567	33.720372
855.722876	45300.078664	33.725389
856.848651	45362.628305	33.730407
858.106380	45434.918030	33.735424
858.602289	45507.174763	33.740442
859.789119	45561.485784	33.745460
860.436476	45628.121116	33.750477
860.924840	45702.163495	33.755495
861.925672	45759.919834	33.760512
862.797551	45835.459083	33.765530
863.629472	45902.857220	33.770548
864.323590	45967.069839	33.775565
865.285058	46038.294293	33.780583
866.634949	46109.376274	33.785600
867.269911	46181.518646	33.790618
868.238309	46248.365206	33.795636
869.140604	46312.103596	33.800653
869.969785	46379.883145	33.805671
871.267707	46443.275656	33.810688
871.690465	46510.258540	33.815706
872.830912	46568.140724	33.820724
874.340416	46626.844919	33.825741
875.071504	46688.940973	33.830759
875.938967	46739.066153	33.835776
876.971178	46806.397867	33.840794
878.103771	46865.446028	33.845812
878.949423	46921.844112	33.850829
879.697126	46980.389470	33.855847
880.336705	47029.209643	33.860864
881.070743	47089.319953	33.865882
881.839134	47143.023047	33.870900
882.882928	47205.729764	33.875917
883.718745	47269.379995	33.880935
884.452592	47327.321099	33.885952
884.717931	47406.743087	33.890970
886.028574	47465.088200	33.895988
887.106936	47524.867717	33.901005
888.205274	47575.211866	33.906023
889.167438	47638.413285	33.911040
890.256303	47688.822424	33.916058
891.156670	47743.740025	33.921076
892.266306	47799.030067	33.926093
892.793140	47857.314742	33.931111
893.182464	47905.764554	33.936128
894.217943	47963.312386	33.941146
894.892209	48015.039407	33.946164
895.777146	48062.191418	33.951181
896.665701	48124.886891	33.956199
897.601371	48188.745587	33.961216
897.930812	48249.997450	33.966234
899.037151	48311.533434	33.971252
899.788855	48367.393021	33.976269
900.250666	48436.747949	33.981287
901.499865	48502.184626	33.986304
902.294234	48571.557789	33.991322
902.906655	48643.053568	33.996340
904.479006	48709.307273	34.001357
905.137289	48784.908615	34.006375
906.169052	48855.605903	34.011392
906.590207	48920.799411	34.016410
907.690821	49001.191451	34.021428
908.615741	49071.191129	34.026445
909.436104	49137.620078	34.031463
910.679473	49208.393073	34.036480
911.604789	49295.677894	34.041498
912.133184	49366.847378	34.046516
913.387980	49432.848936	34.051533
914.184576	49512.050056	34.056551
915.057046	49587.323354	34.061568
916.047408	49659.718829	34.066586
917.006725	49734.915826	34.071604
918.263095	49804.707985	34.076621
919.417726	49875.174189	34.081639
920.407956	49942.724196	34.086656
921.514692	50013.609529	34.091674
922.294899	50078.820040	34.096692
924.047079	50136.812239	34.101709
924.758378	50196.763469	34.106727
925.723816	50253.790193	34.111744
926.758435	50318.999746	34.116762
927.188438	50388.941300	34.121780
928.461295	50445.661240	34.126797
929.031141	50504.932992	34.131815
930.008611	50568.880414	34.136832
931.200206	50637.755113	34.141850
931.957643	50713.347383	34.146868
932.930489	50783.136035	34.151885
933.547937	50844.350003	34.156903
934.641570	50907.217323	34.161920
935.458269	50977.764821	34.166938
936.143687	51050.458907	34.171956
937.357963	51109.290230	34.176973
937.948812	51184.625251	34.181991
938.939527	51259.562929	34.187008
939.729176	51337.834984	34.192026
940.803682	51414.531757	34.197044
942.480943	51473.146411	34.202061
943.229250	51537.866159	34.207079
944.133923	51601.435480	34.212096
945.120210	51668.535595	34.217114
945.795191	51736.816963	34.222132
947.004591	51805.951799	34.227149
947.609720	51870.410030	34.232167
948.601320	51938.522485	34.237184
949.443826	52009.581634	34.242202
950.257295	52084.998823	34.247220
951.403832	52159.579800	34.252237
951.848496	52232.549188	34.257255
952.955580	52305.687776	34.262272
953.905801	52382.691837	34.267290
954.684650	52442.720634	34.272308
955.845682	52512.864861	34.277325
956.360894	52584.868905	34.282343
957.798826	52640.189117	34.287360
958.616992	52706.717276	34.292378
959.322876	52776.040947	34.297396
960.690989	52831.359827	34.302413
961.626373	52905.450867	34.307431
962.730479	52961.019965	34.312448
963.699907	53028.506292	34.317466
964.443321	53096.306417	34.322484
965.361564	53166.895382	34.327501
966.209728	53243.551162	34.332519
967.327298	53317.374693	34.337536
968.574892	53379.168000	34.342554
969.059097	53459.102005	34.347572
970.324930	53524.841436	34.352589
971.070437	53608.709176	34.357607
971.907581	53676.939346	34.362624
973.368997	53746.989900	34.367642
974.094393	53827.260963	34.372660
975.341228	53904.844009	34.377677
976.468931	53967.537120	34.382695
977.280325	54047.770238	34.387712
978.400606	54115.445041	34.392730
979.307253	54184.001250	34.397748
980.496617	54256.240880	34.402765
981.555982	54328.437688	34.407783
982.144450	54395.493662	34.412800
983.791376	54466.498343	34.417818
984.731037	54531.835744	34.422836
986.096719	54596.676696	34.427853
986.775807	54662.630882	34.432871
987.870357	54733.304693	34.437888
989.056697	54801.812837	34.442906
989.887730	54864.371000	34.447924
991.191956	54925.817840	34.452941
992.080028	54995.107050	34.457959
993.207841	55052.189868	34.462976
994.166921	55114.462974	34.467994
994.823546	55193.591321	34.473012
995.710704	55248.838893	34.478029
996.846072	55327.393227	34.483047
997.482939	55390.603186	34.488064
998.673024	55476.243597	34.493082
999.269047	55547.642940	34.498100
1000.304604	55619.087992	34.503117
1001.200945	55699.009735	34.508135
1001.975375	55781.596025	34.513152
1003.795561	55852.913317	34.518170
1004.193935	55936.609212	34.523188
1005.537929	56008.564334	34.528205
1006.480628	56090.828065	34.533223
1007.135614	56167.301920	34.538240
1008.452051	56237.236882	34.543258
1009.252231	56316.960499	34.548276
1010.204637	56394.464652	34.553293
1011.454891	56479.871483	34.558311
1012.368207	56552.173751	34.563328
1013.595184	56629.135962	34.568346
1014.658146	56705.687270	34.573364
1015.675553	56779.638476	34.578381
1016.882680	56846.041820	34.583399
1017.914267	56921.750653	34.588416
1018.690301	56985.791241	34.593434
1019.526440	57062.043573	34.598452
1020.704038	57133.382456	34.603469
1021.762000	57210.986748	34.608487
1022.836713	57276.165116	34.613504
1023.776530	57334.700346	34.618522
1024.637013	57399.716202	34.623540
1025.806191	57458.722345	34.628557
1026.940617	57524.904722	34.633575
1027.768740	57586.305973	34.638592
1028.785253	57658.747417	34.643610
1029.657146	57730.224269	34.648628
1030.506711	57798.211200	34.653645
1031.370321	57876.809908	34.658663
1031.930136	57959.785228	34.663680
1033.110508	58033.037728	34.668698
1034.331877	58105.575213	34.673716
1035.726507	58188.041628	34.678733
1036.571595	58259.017896	34.683751
1037.351040	58354.226234	34.688768
1038.654112	58429.808958	34.693786
1039.782930	58513.811549	34.698804
1041.024909	58597.239847	34.703821
1041.661069	58678.933586	34.708839
1042.383708	58764.823095	34.713856
1043.461004	58841.410628	34.718874
1044.893305	58930.367557	34.723892
1045.933987	59019.581981	34.728909
1046.952063	59105.002645	34.733927
1047.724777	59187.531306	34.738944
1048.591926	59268.672071	34.743962
1049.703371	59364.320068	34.748980
1050.658357	59456.422993	34.753997
1051.958239	59545.877502	34.759015
1052.995086	59643.272482	34.764032
1054.138399	59722.536225	34.769050
1055.550123	59820.557149	34.774068
1056.294824	59905.004126	34.779085
1057.876783	59988.966614	34.784103
1058.613617	60082.713580	34.789120
1060.039464	60163.308304	34.794138
1061.049147	60252.766277	34.799156
1062.311915	60344.349931	34.804173
1063.689820	60420.686772	34.809191
1064.907661	60505.834404	34.814208
1065.999921	60585.001295	34.819226
1066.745013	60668.748255	34.824244
1067.777588	60744.747419	34.829261
1069.261400	60826.518978	34.834279
1070.178822	60907.942217	34.839296
1071.820235	60977.295978	34.844314
1072.616083	61060.637598	34.849332
1073.150254	61138.817077	34.854349
1074.262602	61208.006979	34.859367
1074.891007	61298.129464	34.864384
1076.284687	61388.683862	34.869402
1077.456354	61467.429799	34.874420
1078.527295	61550.673292	34.879437
1079.639416	61639.734259	34.884455
1080.571836	61721.366751	34.889472
1081.574562	61804.748323	34.894490
1082.655631	61894.017603	34.899508
1083.715863	61983.258801	34.904525
1085.081820	62067.027826	34.909543
1085.778745	62153.078843	34.914560
1087.635930	62235.854109	34.919578
1089.003742	62305.646680	34.924596
1089.890135	62381.369811	34.929613
1091.285487	62468.370353	34.934631
1092.050589	62544.555979	34.939648
1093.148819	62616.398075	34.944666
1094.017151	62688.712953	34.949684
1094.795150	62763.643852	34.954701
1095.767392	62831.587735	34.959719
1096.609431	62911.351797	34.964736
1097.918849	62970.754610	34.969754
1098.724886	63058.026205	34.974772
1099.882089	63138.020475	34.979789
1100.870751	63215.755961	34.984807
1101.661818	63305.467961	34.989824
1102.900811	63380.196026	34.994842
1103.872735	63468.215554	34.999860
1104.891302	63555.430491	35.004877
1106.414140	63629.836582	35.009895
1107.407295	63714.998618	35.014912
1108.978480	63792.537613	35.019930
1110.409735	63874.251487	35.024948
1111.678458	63959.744969	35.029965
1113.015916	64025.210649	35.034983
1113.893397	64102.637018	35.040000
1115.230601	64177.675051	35.045018
1115.638914	64264.360724	35.050036
1116.488172	64346.641536	35.055053
1117.941158	64421.997807	35.060071
1118.662535	64522.620185	35.065088
1120.071779	64599.465192	35.070106
1121.549880	64687.878705	35.075124
1122.361240	64789.228848	35.080141
1123.312524	64868.830226	35.085159
1124.530242	64956.709112	35.090176
1125.696848	65043.589655	35.095194
1126.938662	65131.914896	35.100212
1128.012796	65221.811290	35.105229
1129.691800	65304.725798	35.110247
1130.442636	65400.725526	35.115264
1131.564639	65491.280182	35.120282
1132.922961	65577.240057	35.125300
1133.367309	65670.661155	35.130317
1134.940717	65751.922182	35.135335
1135.907067	65855.721599	35.140352
1137.033406	65942.833098	35.145370
1138.250461	66037.376168	35.150388
1139.270879	66129.006220	35.155405
1141.154456	66224.560522	35.160423
1142.324357	66320.973354	35.165440
1143.011941	66394.732592	35.170458
1144.347991	66488.834635	35.175476
1145.542942	66572.613727	35.180493
1147.236433	66660.848685	35.185511
1147.878556	66748.557491	35.190528
1149.236144	66828.044820	35.195546
1150.502125	66924.274044	35.200564
1151.573234	67006.718939	35.205581
1152.944011	67071.497237	35.210599
1154.136486	67159.906886	35.215616
1155.304129	67235.613556	35.220634
1156.559113	67316.916506	35.225652
1157.133223	67404.334249	35.230669
1158.869086	67490.634398	35.235687
1159.575516	67569.845512	35.240704
1160.721495	67652.375814	35.245722
1162.515243	67744.727076	35.250740
1163.243083	67833.635596	35.255757
1164.219124	67909.741321	35.260775
1165.139491	68008.573727	35.265792
1166.420004	68099.182655	35.270810
1167.451295	68187.443665	35.275828
1168.408159	68271.398363	35.280845
1169.703883	68355.294260	35.285863
1170.715360	68459.122588	35.290880
1171.702730	68537.602807	35.295898
1172.844669	68615.451357	35.300916
1173.729436	68712.424146	35.305933
1174.980241	68791.573294	35.310951
1175.944547	68882.234205	35.315968
1177.137741	68974.227485	35.320986
1178.367623	69058.693127	35.326004
1179.451146	69157.504554	35.331021
1180.365515	69242.235193	35.336039
1181.760401	69351.288251	35.341056
1182.916138	69427.908713	35.346074
1184.329884	69517.780056	35.351092
1185.288398	69620.551201	35.356109
1186.716425	69713.308394	35.361127
1188.029872	69809.769005	35.366144
1189.132104	69891.927048	35.371162
1190.610278	70000.627946	35.376180
1191.374650	70094.148340	35.381197
1193.195146	70186.934788	35.386215
1194.612416	70276.364966	35.391232
1195.747607	70368.416556	35.396250
1197.097779	70452.659063	35.401268
1198.365210	70544.044807	35.406285
1200.076184	70632.670627	35.411303
1200.676098	70719.532016	35.416320
1202.175571	70807.760759	35.421338
1203.684664	70891.834308	35.426356
1204.658140	70995.431761	35.431373
1205.640901	71075.307169	35.436391
1206.185027	71172.221863	35.441408
1207.556764	71266.842414	35.446426
1208.814979	71367.332138	35.451444
1209.940597	71463.207534	35.456461
1211.460766	71556.666189	35.461479
1212.500833	71661.864362	35.466496
1213.702560	71761.351190	35.471514
1215.553213	71842.449007	35.476532
1217.223663	71941.420282	35.481549
1218.282571	72027.074702	35.486567
1219.684554	72118.615985	35.491584
1220.320327	72210.922778	35.496602
1221.768953	72303.027379	35.501620
1222.745727	72397.206872	35.506637
1223.922075	72489.911783	35.511655
1224.982857	72590.398920	35.516672
1226.157693	72685.295874	35.521690
1227.276204	72797.743700	35.526708
1228.423065	72888.795416	35.531725
1229.469629	72991.515434	35.536743
1230.789295	73096.359173	35.541760
1231.813027	73202.161322	35.546778
1233.086939	73303.859237	35.551796
1234.073191	73411.479263	35.556813
1235.881647	73511.942182	35.561831
1237.259497	73615.854309	35.566848
1238.230730	73727.303062	35.571866
1239.524706	73828.125910	35.576884
1240.888434	73931.927476	35.581901
1242.520120	74015.041960	35.586919
1244.366032	74118.224557	35.591936
1245.195395	74211.762134	35.596954
1246.694463	74304.081167	35.601972
1247.875014	74398.578036	35.606989
1249.365765	74491.646324	35.612007
1250.566194	74574.829680	35.617024
1251.729683	74665.188240	35.622042
1253.139487	74750.188851	35.627060
1253.748072	74848.892941	35.632077
1254.920762	74933.373713	35.637095
1256.436668	75025.312620	35.642112
1257.355753	75103.512773	35.647130
1258.406437	75179.805336	35.652148
1259.431964	75275.431430	35.657165
1260.485714	75364.986094	35.662183
1261.978765	75457.956048	35.667200
1262.533258	75551.262415	35.672218
1264.037813	75653.972060	35.677236
1265.117736	75760.966283	35.682253
1266.562473	75858.087230	35.687271
1267.918003	75959.301196	35.692288
1268.964414	76063.198411	35.697306
1270.416137	76161.902749	35.702324
1271.689648	76271.376954	35.707341
1272.936408	76373.242761	35.712359
1274.631648	76477.445927	35.717376
1275.350213	76595.684907	35.722394
1277.003012	76693.118487	35.727412
1278.484118	76804.639985	35.732429
1279.767150	76905.083393	35.737447
1280.913534	77009.779395	35.742464
1282.043535	77128.742041	35.747482
1283.911723	77228.601528	35.752500
1285.174482	77318.003449	35.757517
1286.714084	77428.036282	35.762535
1288.560721	77524.593936	35.767552
1289.458972	77615.066989	35.772570
1290.400819	77714.363047	35.777588
1291.948130	77825.422379	35.782605
1293.529871	77916.727470	35.787623
1295.022248	78019.308618	35.792640
1296.134884	78124.951585	35.797658
1297.196501	78214.679115	35.802676
1298.365725	78321.264136	35.807693
1299.429408	78434.871504	35.812711
1300.591958	78542.775915	35.817728
1302.021055	78654.059699	35.822746
1303.432134	78740.263442	35.827764
1304.945335	78862.062357	35.832781
1306.260282	78971.794314	35.837799
1307.453352	79072.563727	35.842816
1308.559491	79187.472446	35.847834
1310.248101	79293.942387	35.852852
1311.250228	79409.374962	35.857869
1312.411627	79519.297688	35.862887
1313.938950	79635.814980	35.867904
1315.025296	79736.565420	35.872922
1316.559707	79850.574093	35.877940
1318.038784	79963.324961	35.882957
1319.443625	80063.963672	35.887975
1321.332230	80175.815510	35.892992
1322.196832	80285.673451	35.898010
1323.793837	80392.161872	35.903028
1325.291836	80495.169433	35.908045
1326.917713	80593.913298	35.913063
1328.017394	80683.642920	35.918080
1329.808019	80786.225934	35.923098
1331.467006	80875.235654	35.928116
1332.509197	80965.025807	35.933133
1333.538841	81054.514136	35.938151
1335.183950	81155.841552	35.943168
1336.271137	81256.445329	35.948186
1337.630988	81337.521318	35.953204
1339.223111	81432.497891	35.958221
1340.592456	81522.618999	35.963239
1341.759714	81615.153742	35.968256
1342.984802	81712.620963	35.973274
1344.067456	81795.679884	35.978292
1345.590593	81874.134718	35.983309
1346.580596	81962.947952	35.988327
1347.930530	82046.776879	35.993344
1348.946791	82137.360353	35.998362
1350.135848	82231.186058	36.003380
1351.200282	82318.468439	36.008397
1352.395109	82421.023474	36.013415
1353.766630	82513.871470	36.018432
1355.099616	82631.267722	36.023450
1356.435540	82722.994308	36.028468
1357.573826	82831.894702	36.033485
1358.936780	82930.320278	36.038503
1360.340141	83041.410178	36.043520
1361.754733	83161.494696	36.048538
1363.143839	83255.051925	36.053556
1364.685363	83359.482294	36.058573
1365.695437	83478.123334	36.063591
1367.288698	83592.391460	36.068608
1368.694898	83707.829513	36.073626
1370.237752	83813.997212	36.078644
1371.359236	83929.961964	36.083661
1372.372431	84042.003449	36.088679
1374.228310	84160.908474	36.093696
1375.687149	84277.557033	36.098714
1377.229296	84391.278800	36.103732
1378.008329	84510.416243	36.108749
1379.429923	84634.852004	36.113767
1380.973151	84758.103637	36.118784
1381.907135	84886.100918	36.123802
1383.330265	85008.383973	36.128820
1385.383947	85139.363216	36.133837
1386.428096	85258.994688	36.138855
1388.370427	85377.992674	36.143872
1389.727995	85499.692470	36.148890
1391.395057	85617.087012	36.153908
1392.612397	85735.857191	36.158925
1394.251807	85850.025761	36.163943
1395.482304	85961.039852	36.168960
1397.089225	86083.805722	36.173978
1398.494399	86205.615124	36.178996
1400.144426	86312.865137	36.184013
1401.021019	86429.625707	36.189031
1402.903348	86545.723333	36.194048
1403.825725	86673.895067	36.199066
1405.099920	86794.130667	36.204084
1406.755139	86921.264373	36.209101
1407.606229	87046.014732	36.214119
1409.432705	87166.685460	36.219136
1411.219556	87287.375527	36.224154
1412.485463	87397.578571	36.229172
1414.147873	87520.367208	36.234189
1415.544914	87640.599844	36.239207
1417.195325	87749.527826	36.244224
1418.606391	87872.344386	36.249242
1420.233494	87975.384174	36.254260
1421.934669	88089.703976	36.259277
1422.847178	88203.766802	36.264295
1424.554490	88315.767454	36.269312
1425.911044	88435.274635	36.274330
1427.328433	88541.694624	36.279348
1428.603974	88661.278694	36.284365
1429.932335	88763.556685	36.289383
1431.708780	88870.973815	36.294400
1433.150751	88991.648526	36.299418
1434.432267	89098.928080	36.304436
1435.775451	89210.849403	36.309453
1437.138552	89311.387684	36.314471
1438.612177	89414.076196	36.319488
1439.998129	89509.884546	36.324506
1441.697740	89611.309276	36.329524
1443.035543	89709.964548	36.334541
1444.073078	89804.687493	36.339559
1445.593899	89908.739076	36.344576
1446.448096	90011.259924	36.349594
1447.598771	90117.575003	36.354612
1449.480440	90225.132737	36.359629
1450.985548	90347.336605	36.364647
1452.448884	90457.887857	36.369664
1453.756255	90565.422143	36.374682
1454.825765	90690.673494	36.379700
1456.049504	90806.079289	36.384717
1456.950329	90947.288738	36.389735
1458.798983	91065.906102	36.394752
1460.138943	91193.233971	36.399770
1462.180199	91316.663740	36.404788
1464.017209	91440.138480	36.409805
1465.563306	91561.605825	36.414823
1467.361392	91675.518751	36.419840
1468.833799	91795.756455	36.424858
1470.137299	91915.564660	36.429876
1471.871901	92027.689072	36.434893
1472.917745	92164.280926	36.439911
1474.686157	92283.384514	36.444928
1476.071952	92408.467026	36.449946
1477.485294	92527.170561	36.454964
1479.431063	92648.022385	36.459981
1480.620910	92771.628636	36.464999
1482.596872	92887.318205	36.470016
1483.884297	93018.350209	36.475034
1485.332288	93132.082279	36.480052
1487.200799	93248.157507	36.485069
1487.964794	93381.490604	36.490087
1490.130705	93503.997296	36.495104
1491.245200	93620.280019	36.500122
1492.534489	93750.288208	36.505140
1494.312883	93870.473806	36.510157
1495.609373	94004.221051	36.515175
1497.486025	94128.346957	36.520192
1499.054266	94262.091051	36.525210
1500.255586	94387.996228	36.530228
1501.982835	94501.575835	36.535245
1502.815446	94634.852985	36.540263
1505.026385	94767.624648	36.545280
1506.799656	94891.389459	36.550298
1507.856680	95010.322845	36.555316
1509.705580	95150.973218	36.560333
1510.728004	95269.317236	36.565351
1512.648735	95392.642807	36.570368
1514.264220	95518.348687	36.575386
1515.517435	95641.943927	36.580404
1517.158084	95765.213164	36.585421
1518.421237	95901.724422	36.590439
1520.111666	96026.343250	36.595456
1521.829037	96149.690797	36.600474
1523.191694	96286.391062	36.605492
1524.678746	96398.455858	36.610509
1526.149551	96537.003749	36.615527
1527.593316	96658.101529	36.620544
1529.298531	96793.825338	36.625562
1530.701514	96927.568589	36.630580
1532.115316	97056.937430	36.635597
1533.756700	97183.761479	36.640615
1535.266606	97321.406728	36.645632
1536.626579	97448.579874	36.650650
1538.399946	97559.374637	36.655668
1540.400967	97681.302321	36.660685
1541.471207	97787.542383	36.665703
1542.936653	97902.582200	36.670720
1544.215942	98011.477906	36.675738
1545.713869	98134.449061	36.680756
1547.299765	98241.003359	36.685773
1548.398156	98369.906919	36.690791
1550.107875	98487.078558	36.695808
1552.078868	98611.106162	36.700826
1553.046782	98734.605821	36.705844
1554.845714	98842.853034	36.710861
1556.333219	98989.851905	36.715879
1557.339373	99117.961517	36.720896
1559.202947	99252.200672	36.725914
1560.493548	99382.663041	36.730932
1562.032604	99520.199176	36.735949
1563.709828	99653.023814	36.740967
1565.187668	99797.936149	36.745984
1566.623417	99941.258340	36.751002
1568.078079	100089.459031	36.756020
1570.046249	100225.967911	36.761037
1571.591550	100367.981845	36.766055
1573.350645	100507.960069	36.771072
1575.214340	100646.578789	36.776090
1576.716680	100795.700766	36.781108
1578.757037	100928.131835	36.786125
1580.699734	101057.599362	36.791143
1582.146053	101195.537400	36.796160
1583.935363	101332.623931	36.801178
1585.390868	101464.742522	36.806196
1587.043770	101585.826416	36.811213
1588.481411	101722.246674	36.816231
1590.460532	101852.789329	36.821248
1592.073560	101991.186553	36.826266
1593.153537	102128.982704	36.831284
1595.405309	102259.332406	36.836301
1596.893420	102403.595494	36.841319
1598.480766	102532.667758	36.846336
1599.993587	102661.625344	36.851354
1601.148908	102803.190765	36.856372
1603.099768	102948.690102	36.861389
1604.334911	103093.211118	36.866407
1605.726138	103227.857171	36.871424
1607.357677	103372.178245	36.876442
1608.807063	103521.637835	36.881460
1610.658341	103657.748160	36.886477
1612.288984	103809.982852	36.891495
1614.302881	103961.156956	36.896512
1615.972783	104091.858036	36.901530
1617.137424	104249.479755	36.906548
1618.859865	104392.447135	36.911565
1620.639337	104533.073289	36.916583
1622.204498	104685.347529	36.921600
1624.129784	104822.909201	36.926618
1625.655452	104964.096519	36.931636
1627.881414	105094.207799	36.936653
1629.453815	105229.531102	36.941671
1631.054397	105366.308701	36.946688
1632.887243	105500.895190	36.951706
1634.561828	105639.805216	36.956724
1636.289869	105774.903614	36.961741
1638.028036	105914.362776	36.966759
1639.393919	106037.650438	36.971776
1641.061771	106168.144364	36.976794
1642.320471	106307.020422	36.981812
1643.748870	106440.329541	36.986829
1645.163492	106583.531650	36.991847
1646.604822	106724.232254	36.996864
1648.354435	106859.965614	37.001882
1649.575033	106992.332876	37.006900
1651.178397	107119.137913	37.011917
1652.424879	107243.336135	37.016935
1654.178520	107379.311856	37.021952
1655.971385	107513.215131	37.026970
1657.392160	107657.663450	37.031988
1659.373094	107798.931186	37.037005
1660.943257	107944.853743	37.042023
1662.575656	108086.240308	37.047040
1664.002981	108226.315237	37.052058
1665.389839	108373.586912	37.057076
1666.981607	108524.276450	37.062093
1668.624990	108680.462025	37.067111
1670.451709	108837.507420	37.072128
1671.702438	108991.422254	37.077146
1673.387777	109156.949187	37.082164
1675.400012	109316.605491	37.087181
1677.190269	109463.882414	37.092199
1678.833296	109626.996103	37.097216
1680.895206	109794.826125	37.102234
1682.145611	109956.430006	37.107252
1684.181263	110117.316398	37.112269
1685.967754	110280.055728	37.117287
1687.959752	110437.742026	37.122304
1689.791784	110592.727435	37.127322
1691.499055	110742.749144	37.132340
1693.306482	110894.379132	37.137357
1695.266507	111045.846525	37.142375
1696.433948	111209.206438	37.147392
1698.639327	111362.691418	37.152410
1700.687718	111517.000444	37.157428
1702.516240	111655.086355	37.162445
1704.346711	111801.821487	37.167463
1705.904150	111961.421076	37.172480
1708.288751	112107.424448	37.177498
1709.798946	112252.423135	37.182516
1711.552252	112397.879171	37.187533
1713.049357	112541.067537	37.192551
1714.519245	112702.903425	37.197568
1716.112015	112849.388167	37.202586
1718.081290	113001.800918	37.207604
1719.853465	113148.068722	37.212621
1721.408691	113306.736158	37.217639
1722.860783	113458.559172	37.222656
1724.720561	113619.120987	37.227674
1725.981375	113778.609947	37.232692
1727.849930	113932.031537	37.237709
1729.494607	114095.736167	37.242727
1731.228835	114259.858808	37.247744
1733.241852	114415.707712	37.252762
1734.669999	114585.396443	37.257780
1736.381149	114747.444896	37.262797
1738.068132	114919.022682	37.267815
1739.653008	115084.275687	37.272832
1741.700624	115250.928645	37.277850
1742.987021	115429.813167	37.282868
1744.838461	115591.475707	37.287885
1747.039723	115763.357890	37.292903
1748.240294	115930.576989	37.297920
1750.181043	116091.073643	37.302938
1751.631670	116269.137625	37.307956
1753.395945	116445.200399	37.312973
1755.514796	116625.889026	37.317991
1756.840533	116788.424992	37.323008
1759.150443	116956.465372	37.328026
1760.704236	117130.293784	37.333044
1762.706195	117288.160566	37.338061
1764.312243	117441.257121	37.343079
1765.628505	117599.992965	37.348096
1767.659108	117745.985173	37.353114
1769.100774	117898.652560	37.358132
1771.247051	118049.435147	37.363149
1772.698031	118209.852249	37.368167
1774.394419	118371.462192	37.373184
1776.472691	118534.078856	37.378202
1777.714449	118692.234741	37.383220
1779.218174	118857.314157	37.388237
1781.237790	119016.935860	37.393255
1783.250866	119184.930916	37.398272
1785.042539	119351.667364	37.403290
1786.806710	119510.430302	37.408308
1788.472592	119669.856106	37.413325
1790.667260	119843.838256	37.418343
1791.909074	120025.808591	37.423360
1793.681014	120190.306587	37.428378
1795.455164	120378.905936	37.433396
1796.772038	120558.431639	37.438413
1798.835180	120726.324182	37.443431
1800.688705	120928.055368	37.448448
1802.694184	121109.493358	37.453466
1804.280179	121302.071522	37.458484
1805.890703	121475.834821	37.463501
1807.968058	121674.630162	37.468519
1809.897715	121861.538081	37.473536
1812.110587	122047.514845	37.478554
1813.946024	122233.449753	37.483572
1815.310801	122411.961724	37.488589
1817.605092	122607.023902	37.493607
1819.460514	122803.601502	37.498624
1821.744846	122978.966457	37.503642
1823.230997	123164.782529	37.508660
1825.009523	123355.108135	37.513677
1826.665332	123544.844838	37.518695
1828.456199	123734.726341	37.523712
1830.226558	123925.081321	37.528730
1832.052021	124129.154825	37.533748
1834.056697	124323.217589	37.538765
1836.503022	124512.100071	37.543783
1838.281649	124698.588195	37.548800
1840.119123	124886.996326	37.553818
1841.996527	125077.175199	37.558836
1844.122709	125257.674657	37.563853
1846.155831	125435.246171	37.568871
1847.697543	125638.978223	37.573888
1849.764761	125832.619872	37.578906
1851.592666	126005.417645	37.583924
1853.349731	126186.092865	37.588941
1855.451815	126374.454043	37.593959
1856.949427	126551.695119	37.598976
1859.269267	126734.213553	37.603994
1861.175021	126922.036904	37.609012
1863.328084	127085.032470	37.614029
1865.477916	127266.196860	37.619047
1867.460115	127442.871571	37.624064
1869.430821	127617.531588	37.629082
1870.802350	127795.863355	37.634100
1872.766455	127973.862607	37.639117
1874.455182	128137.886130	37.644135
1876.208308	128325.561992	37.649152
1877.978913	128498.607516	37.654170
1879.798101	128684.193992	37.659188
1881.344943	128873.896339	37.664205
1882.907651	129055.210656	37.669223
1884.378359	129251.282981	37.674240
1886.647351	129437.703599	37.679258
1888.458125	129615.238881	37.684276
1890.609526	129783.459882	37.689293
1892.508651	129948.460065	37.694311
1894.061899	130122.535741	37.699328
1895.671042	130287.189052	37.704346
1897.592208	130474.708774	37.709364
1899.133650	130656.502713	37.714381
1900.981380	130831.182539	37.719399
1902.677623	131021.695972	37.724416
1904.779704	131203.798311	37.729434
1906.225912	131403.005645	37.734452
1908.405462	131590.033261	37.739469
1910.801555	131774.591837	37.744487
1912.317885	131979.183437	37.749504
1913.897606	132168.869958	37.754522
1916.169298	132373.904148	37.759540
1917.518184	132577.040075	37.764557
1919.898573	132787.185454	37.769575
1921.680209	132992.095805	37.774592
1923.259398	133205.895331	37.779610
1925.311348	133398.444787	37.784628
1926.883944	133617.284775	37.789645
1928.994160	133832.019802	37.794663
1931.038452	134059.010959	37.799680
1933.311772	134274.585596	37.804698
1934.753043	134490.151197	37.809716
1937.011434	134717.962567	37.814733
1939.227839	134937.800133	37.819751
1941.294292	135160.859809	37.824768
1943.193806	135372.297784	37.829786
1945.321721	135580.934923	37.834804
1947.016902	135805.895542	37.839821
1949.167768	136029.187482	37.844839
1950.899193	136253.865518	37.849856
1953.367652	136472.275490	37.854874
1955.666472	136678.848061	37.859892
1957.031475	136910.362654	37.864909
1959.659562	137123.713074	37.869927
1961.626720	137350.555158	37.874944
1962.811347	137563.637370	37.879962
1965.073952	137782.821648	37.884980
1966.746689	138010.258469	37.889997
1969.313461	138227.278277	37.895015
1971.175065	138461.096419	37.900032
1973.048986	138672.908959	37.905050
1975.633800	138898.507684	37.910068
1976.846605	139126.694125	37.915085
1979.067920	139344.978480	37.920103
1981.165460	139583.194462	37.925120
1983.176200	139801.945184	37.930138
1984.984472	140028.215878	37.935156
1986.858620	140257.129746	37.940173
1988.962249	140485.932857	37.945191
1991.106280	140695.758073	37.950208
1993.599962	140924.375673	37.955226
1995.882639	141144.321254	37.960244
1998.072071	141366.757089	37.965261
1999.765991	141583.090549	37.970279
2001.769281	141795.531440	37.975296
2003.673235	142019.169596	37.980314
2005.871751	142238.308337	37.985332
2007.549753	142457.237175	37.990349
2009.864825	142662.843524	37.995367
2011.798993	142878.498104	38.000384
2013.480594	143099.840612	38.005402
2015.645764	143322.378002	38.010420
2017.568934	143540.270892	38.015437
2020.215660	143751.693658	38.020455
2022.125471	143941.085142	38.025472
2023.739373	144124.736004	38.030490
2026.117733	144318.663078	38.035508
2027.944273	144506.622818	38.040525
2029.720950	144696.685173	38.045543
2031.918801	144902.623672	38.050560
2033.421360	145110.778082	38.055578
2035.529227	145313.978124	38.060596
2037.081623	145514.993562	38.065613
2038.894468	145730.552445	38.070631
2040.459936	145964.249708	38.075648
2042.282524	146188.046202	38.080666
2044.166603	146408.597585	38.085684
2045.631096	146648.139426	38.090701
2047.389823	146878.751943	38.095719
2049.804296	147133.277476	38.100736
2051.908007	147383.181796	38.105754
2053.862261	147632.120563	38.110772
2055.513470	147880.422283	38.115789
2058.049672	148135.009934	38.120807
2059.950112	148398.785754	38.125824
2062.193967	148677.639252	38.130842
2064.144626	148934.847770	38.135860
2066.437651	149188.069453	38.140877
2068.420304	149450.961919	38.145895
2070.642920	149706.367525	38.150912
2072.741265	149976.111503	38.155930
2075.119150	150229.248759	38.160948
2077.242357	150488.265721	38.165965
2079.208005	150747.790790	38.170983
2081.284332	151015.512467	38.176000
2083.349497	151287.882984	38.181018
2085.956173	151545.763500	38.186036
2087.868880	151813.666876	38.191053
2090.564882	152071.104378	38.196071
2093.052373	152327.217312	38.201088
2094.630042	152593.615297	38.206106
2097.455935	152836.984217	38.211124
2099.858387	153090.879804	38.216141
2101.888053	153332.204157	38.221159
2104.228923	153585.311855	38.226176
2106.278322	153840.002024	38.231194
2108.816335	154073.291307	38.236212
2110.723330	154327.142634	38.241229
2112.642809	154569.898462	38.246247
2114.812163	154827.811396	38.251264
2116.540319	155073.734606	38.256282
2118.718390	155324.247658	38.261300
2120.740376	155583.494428	38.266317
2123.211380	155835.322403	38.271335
2125.364499	156086.604300	38.276352
2127.381826	156340.180734	38.281370
2129.238164	156602.771091	38.286388
2131.187296	156858.797740	38.291405
2133.213430	157110.014917	38.296423
2135.513295	157371.105164	38.301440
2137.395608	157631.195177	38.306458
2140.081357	157891.935669	38.311476
2141.758135	158149.851016	38.316493
2144.066908	158410.627041	38.321511
2145.908618	158676.859574	38.326528
2147.743530	158942.459580	38.331546
2150.239433	159209.176607	38.336564
2152.236676	159485.290683	38.341581
2154.179458	159749.734838	38.346599
2156.262186	160013.218896	38.351616
2158.186569	160287.735600	38.356634
2160.792504	160543.942213	38.361652
2162.755874	160800.681528	38.366669
2165.006438	161037.419841	38.371687
2167.334272	161270.579566	38.376704
2169.201378	161517.611988	38.381722
2171.601526	161771.430771	38.386740
2173.464310	162017.678682	38.391757
2175.237514	162277.068904	38.396775
2177.674437	162528.840958	38.401792
2179.480224	162788.444004	38.406810
2181.714991	163039.868639	38.411828
2183.566694	163317.126680	38.416845
2185.911363	163580.203898	38.421863
2188.030979	163846.288081	38.426880
2190.238425	164117.958662	38.431898
2192.387211	164384.180135	38.436916
2194.521231	164669.170001	38.441933
2196.697980	164947.895169	38.446951
2199.198640	165238.378681	38.451968
2200.729002	165520.749104	38.456986
2203.495347	165791.171445	38.462004
2205.519229	166078.711019	38.467021
2207.914230	166363.197662	38.472039
2210.345159	166639.465195	38.477056
2212.803253	166927.639069	38.482074
2215.008508	167207.727602	38.487092
2217.274250	167494.486344	38.492109
2219.612576	167784.053658	38.497127
2221.803280	168073.505476	38.502144
2223.849023	168356.213587	38.507162
2226.456720	168635.762704	38.512180
2228.580833	168937.874589	38.517197
2230.899720	169225.939873	38.522215
2233.297736	169510.222951	38.527232
2234.739934	169812.901729	38.532250
2237.577611	170104.279915	38.537268
2239.876411	170409.811704	38.542285
2242.096832	170706.049821	38.547303
2244.411473	171002.071305	38.552320
2246.224320	171309.396585	38.557338
2248.246947	171597.771240	38.562356
2250.660103	171913.208139	38.567373
2252.813039	172211.430841	38.572391
2255.771042	172496.730216	38.577408
2258.411836	172806.561140	38.582426
2260.801621	173108.432809	38.587444
2262.831435	173406.971372	38.592461
2264.884564	173698.726816	38.597479
2267.418824	174001.671483	38.602496
2269.346732	174300.394389	38.607514
2271.825752	174591.934491	38.612532
2274.307778	174904.350729	38.617549
2276.499691	175196.978962	38.622567
2278.951961	175498.938944	38.627584
2281.209921	175806.682557	38.632602
2283.820334	176100.099700	38.637620
2285.902058	176390.933540	38.642637
2288.274846	176684.224672	38.647655
2290.447334	176974.487714	38.652672
2292.710735	177265.131267	38.657690
2295.206959	177560.945948	38.662708
2297.324897	177866.141214	38.667725
2299.647072	178151.470711	38.672743
2302.226080	178451.948664	38.677760
2304.135309	178754.563679	38.682778
2306.961958	179044.084357	38.687796
2309.367632	179343.957450	38.692813
2311.322911	179640.726979	38.697831
2313.318124	179935.992836	38.702848
2315.469479	180215.438049	38.707866
2317.522901	180486.111771	38.712884
2319.562011	180776.801988	38.717901
2321.760491	181054.744006	38.722919
2323.878921	181334.451788	38.727936
2326.125192	181630.725437	38.732954
2328.581019	181911.703165	38.737972
2330.974078	182199.701410	38.742989
2332.861013	182492.960553	38.748007
2335.095386	182790.738240	38.753024
2337.138755	183092.330953	38.758042
2339.506602	183404.135115	38.763060
2341.829663	183710.359571	38.768077
2344.082562	184041.842186	38.773095
2346.641144	184354.508679	38.778112
2348.646776	184667.338417	38.783130
2351.382657	184982.163606	38.788148
2353.284844	185311.114376	38.793165
2355.608642	185637.409902	38.798183
2358.254323	185954.944475	38.803200
2360.548194	186298.797593	38.808218
2362.798717	186652.361146	38.813236
2365.187300	187037.171092	38.818253
2367.419341	187369.810828	38.823271
2370.160701	187701.051565	38.828288
2372.699436	188045.456486	38.833306
2375.575077	188374.062237	38.838324
2378.102541	188709.987512	38.843341
2380.290614	189042.563048	38.848359
2382.872634	189367.331283	38.853376
2384.931515	189713.390909	38.858394
2387.634779	190039.945623	38.863412
2390.492577	190372.649470	38.868429
2392.936246	190696.477837	38.873447
2395.676680	191026.839609	38.878464
2397.996735	191361.662004	38.883482
2400.956812	191686.657361	38.888500
2403.224962	192010.262653	38.893517
2405.402156	192344.398821	38.898535
2408.187989	192668.306315	38.903552
2410.209838	192999.801376	38.908570
2412.472443	193322.598177	38.913588
2414.983129	193654.095103	38.918605
2417.046108	193995.264128	38.923623
2419.663762	194335.484106	38.928640
2422.331533	194671.658406	38.933658
2424.743490	195007.771777	38.938676
2427.481394	195338.043801	38.943693
2429.708358	195676.245147	38.948711
2431.956722	196006.340984	38.953728
2434.659641	196337.509940	38.958746
2436.660353	196680.676852	38.963764
2439.453401	197006.651478	38.968781
2441.600452	197349.949657	38.973799
2444.322584	197689.729940	38.978816
2446.840098	198035.258246	38.983834
2449.010931	198365.803478	38.988852
2451.496461	198702.676326	38.993869
2453.824245	199053.723319	38.998887
2456.248028	199393.833352	39.003904
2458.782458	199737.025957	39.008922
2461.479930	200076.383637	39.013940
2463.846589	200414.015381	39.018957
2466.086593	200755.579476	39.023975
2468.163678	201105.171333	39.028992
2471.241357	201450.899487	39.034010
2473.472091	201805.981196	39.039028
2475.690885	202139.092469	39.044045
2477.904695	202470.096762	39.049063
2480.014793	202796.367565	39.054080
2482.291037	203128.201662	39.059098
2484.349391	203457.580831	39.064116
2486.918479	203796.305473	39.069133
2489.028385	204140.487554	39.074151
2491.174783	204481.895692	39.079168
2493.594546	204833.600809	39.084186
2496.380370	205188.678968	39.089204
2499.065497	205533.866338	39.094221
2501.461571	205891.572089	39.099239
2503.933128	206236.108014	39.104256
2506.307529	206603.496878	39.109274
2508.779631	206963.529710	39.114292
2511.905996	207331.869726	39.119309
2514.176270	207694.602490	39.124327
2517.362285	208045.177655	39.129344
2520.087137	208405.935580	39.134362
2522.665124	208761.610874	39.139380
2525.374028	209126.690922	39.144397
2527.761893	209491.948493	39.149415
2530.369016	209844.140582	39.154432
2532.538968	210209.560121	39.159450
2535.041610	210588.036538	39.164468
2537.506710	210951.556724	39.169485
2540.053626	211333.456752	39.174503
2542.650061	211702.165188	39.179520
2545.284734	212079.378319	39.184538
2548.292659	212440.580420	39.189556
2551.082995	212812.486311	39.194573
2553.773397	213190.251023	39.199591
2556.728619	213551.411799	39.204608
2559.146127	213926.628659	39.209626
2561.540716	214294.888887	39.214644
2564.109678	214667.136148	39.219661
2566.529603	215052.439099	39.224679
2569.095250	215421.054897	39.229696
2571.922223	215793.085288	39.234714
2574.491926	216174.530062	39.239732
2577.177358	216546.430733	39.244749
2580.728156	216916.520395	39.249767
2583.429170	217263.498060	39.254784
2586.188693	217631.323465	39.259802
2588.823648	217994.443401	39.264820
2591.656839	218352.883822	39.269837
2593.681525	218724.253887	39.274855
2596.627877	219079.247631	39.279872
2599.007974	219433.237334	39.284890
2601.308985	219802.456529	39.289908
2604.025638	220174.202450	39.294925
2606.468308	220548.836450	39.299943
2608.603141	220909.978193	39.304960
2611.022440	221290.738547	39.309978
2613.702747	221675.650110	39.314996
2616.277421	222055.218008	39.320013
2618.535295	222435.724482	39.325031
2621.270149	222818.367003	39.330048
2623.683403	223207.207466	39.335066
2626.437264	223598.789470	39.340084
2628.789659	223986.394784	39.345101
2631.277458	224381.498705	39.350119
2633.789855	224776.878299	39.355136
2636.861946	225173.745887	39.360154
2638.812351	225573.303064	39.365172
2641.458486	225957.128461	39.370189
2643.877786	226380.340100	39.375207
2646.621393	226777.411240	39.380224
2649.733090	227162.231096	39.385242
2652.213108	227537.038379	39.390260
2655.074639	227904.825512	39.395277
2657.654376	228277.991287	39.400295
2660.491337	228636.128544	39.405312
2663.352621	229010.723764	39.410330
2665.829770	229379.484912	39.415348
2668.588451	229752.241374	39.420365
2670.659389	230124.672861	39.425383
2673.372636	230506.073484	39.430400
2675.838712	230877.299989	39.435418
2678.342476	231269.453360	39.440436
2680.869324	231652.787749	39.445453
2683.241296	232053.750986	39.450471
2685.894482	232454.187541	39.455488
2688.424771	232856.853104	39.460506
2691.173877	233265.886124	39.465524
2693.704883	233680.262197	39.470541
2695.926285	234099.157204	39.475559
2698.988152	234528.870127	39.480576
2701.541701	234952.132975	39.485594
2704.403566	235374.483712	39.490612
2707.271673	235809.585762	39.495629
2709.758202	236232.705348	39.500647
2712.730900	236666.037332	39.505664
2715.526363	237101.860557	39.510682
2718.173147	237536.817267	39.515700
2721.257986	237960.324433	39.520717
2724.102092	238402.311547	39.525735
2727.106933	238833.374914	39.530752
2730.166977	239260.796392	39.535770
2733.187339	239687.893198	39.540788
2736.112747	240112.463815	39.545805
2738.932472	240536.008707	39.550823
2741.572928	240965.194998	39.555840
2744.467212	241388.091883	39.560858
2747.125371	241827.994238	39.565876
2750.012818	242253.456504	39.570893
2752.489623	242689.346458	39.575911
2755.185782	243129.799464	39.580928
2757.922682	243568.644911	39.585946
2760.748578	244004.782946	39.590964
2763.638539	244440.376701	39.595981
2766.794748	244881.338989	39.600999
2769.344328	245324.782646	39.606016
2772.340320	245755.886311	39.611034
2774.854602	246194.608666	39.616052
2778.000572	246633.866826	39.621069
2780.817664	247071.727229	39.626087
2783.311087	247509.891029	39.631104
2786.437031	247945.237300	39.636122
2788.988020	248384.660214	39.641140
2791.963734	248817.030289	39.646157
2794.807418	249265.448767	39.651175
2797.623672	249700.280114	39.656192
2800.381675	250136.313326	39.661210
2802.946565	250589.953775	39.666228
2805.621847	251028.486936	39.671245
2808.601338	251468.571898	39.676263
2811.343291	251917.938930	39.681280
2814.410866	252353.816388	39.686298
2817.271418	252803.873649	39.691316
2820.554348	253233.491630	39.696333
2823.168524	253680.206170	39.701351
2825.861163	254110.624706	39.706368
2828.861464	254554.837915	39.711386
2831.417856	254993.276482	39.716404
2834.025635	255432.264507	39.721421
2837.581368	255863.483228	39.726439
2839.980468	256267.929885	39.731456
2842.981394	256665.347155	39.736474
2845.288814	257071.939332	39.741492
2848.423321	257479.163563	39.746509
2851.146787	257883.351563	39.751527
2853.307295	258297.608408	39.756544
2856.232292	258711.059099	39.761562
2858.839808	259140.839634	39.766580
2861.664330	259567.968633	39.771597
2864.366663	260004.386308	39.776615
2867.064933	260443.800264	39.781632
2869.723811	260875.293826	39.786650
2872.001992	261328.866988	39.791668
2874.461909	261780.911475	39.796685
2877.594118	262245.752727	39.801703
2880.329198	262704.786482	39.806720
2883.209469	263169.459885	39.811738
2886.067734	263646.123371	39.816756
2888.800805	264109.418677	39.821773
2891.684270	264588.791801	39.826791
2894.779293	265069.552182	39.831808
2897.684736	265545.945781	39.836826
2900.566526	266035.014988	39.841844
2904.161870	266524.859760	39.846861
2907.305827	267006.238375	39.851879
2910.033487	267492.251201	39.856896
2913.424200	267962.919287	39.861914
2916.393273	268447.162674	39.866932
2919.169103	268931.713065	39.871949
2922.653383	269409.140827	39.876967
2925.335430	269896.545441	39.881984
2928.616727	270381.720811	39.887002
2931.594212	270865.239235	39.892020
2934.437902	271356.014229	39.897037
2937.598298	271845.441978	39.902055
2940.331207	272330.514405	39.907072
2943.627684	272812.753547	39.912090
2946.421233	273299.995310	39.917108
2949.452952	273784.124217	39.922125
2952.633267	274278.487550	39.927143
2956.011178	274769.312493	39.932160
2958.776189	275253.220488	39.937178
2961.899377	275736.257224	39.942196
2964.710725	276219.695179	39.947213
2967.353070	276704.350160	39.952231
2970.363520	277204.766569	39.957248
2973.633834	277694.346198	39.962266
2976.119741	278188.235115	39.967284
2978.832444	278689.653440	39.972301
2981.887914	279188.958151	39.977319
2984.623881	279708.269847	39.982336
2988.043305	280199.689604	39.987354
2990.940521	280711.884111	39.992372
2994.038921	281205.607333	39.997389
2997.221684	281716.531509	40.002407
3000.194106	282207.982088	40.007424
3003.800584	282704.460254	40.012442
3006.798195	283200.445671	40.017460
3009.442315	283689.677129	40.022477
3013.101080	284190.479095	40.027495
3016.255081	284681.401837	40.032512
3019.566154	285162.240971	40.037530
3022.649053	285655.757945	40.042548
3025.535918	286132.390257	40.047565
3028.795860	286617.670815	40.052583
3031.439339	287097.508246	40.057600
3034.968956	287580.378349	40.062618
3037.706281	288055.953733	40.067636
3040.482995	288499.728909	40.072653
3043.683012	288943.816060	40.077671
3046.463313	289386.670503	40.082688
3049.687716	289839.507755	40.087706
3052.401944	290280.918976	40.092724
3055.681115	290726.911146	40.097741
3058.354322	291176.701504	40.102759
3061.054980	291642.023411	40.107776
3064.219906	292097.900505	40.112794
3067.091413	292557.856929	40.117812
3069.670118	293035.399980	40.122829
3072.621240	293503.944090	40.127847
3075.859921	293990.771134	40.132864
3078.786616	294477.084195	40.137882
3081.391360	294962.808643	40.142900
3084.394476	295446.740643	40.147917
3087.902210	295938.816091	40.152935
3090.932197	296454.344605	40.157952
3093.843665	296949.855542	40.162970
3096.937226	297468.741721	40.167988
3099.960296	297975.803374	40.173005
3102.960290	298490.886572	40.178023
3105.530772	299012.784936	40.183040
3108.726540	299543.974369	40.188058
3111.822657	300071.264615	40.193076
3114.138437	300605.830278	40.198093
3117.879108	301147.480264	40.203111
3120.723980	301698.809433	40.208128
3124.076059	302249.800155	40.213146
3127.402669	302793.630389	40.218164
3130.282064	303339.631618	40.223181
3133.893842	303890.310999	40.228199
3136.750165	304453.109172	40.233216
3139.994651	305006.956223	40.238234
3143.442609	305563.253313	40.243252
3146.680830	306111.606394	40.248269
3150.626957	306672.890646	40.253287
3153.885842	307227.955102	40.258304
3157.305396	307770.296797	40.263322
3161.237516	308322.655217	40.268340
3164.236848	308847.942413	40.273357
3167.803235	309386.385346	40.278375
3171.150441	309923.561952	40.283392
3174.699297	310447.781875	40.288410
3177.781142	310984.023467	40.293428
3180.650774	311518.921483	40.298445
3183.847478	312057.696633	40.303463
3186.824888	312606.677412	40.308480
3190.021868	313134.678792	40.313498
3193.083447	313685.004362	40.318516
3195.780036	314230.075823	40.323533
3199.385731	314764.949091	40.328551
3202.684223	315315.472114	40.333568
3205.475890	315849.723348	40.338586
3208.817261	316408.576086	40.343604
3212.356535	316955.082626	40.348621
3215.970909	317494.947149	40.353639
3218.986931	318041.597918	40.358656
3222.328412	318573.751575	40.363674
3225.894233	319110.254094	40.368692
3229.222733	319655.567289	40.373709
3232.846760	320195.879246	40.378727
3235.417991	320724.167750	40.383744
3238.815303	321259.984681	40.388762
3242.055083	321797.138917	40.393780
3245.233860	322325.998181	40.398797
3248.611801	322847.867124	40.403815
3251.584534	323373.446558	40.408832
3255.008204	323865.810523	40.413850
3258.365323	324363.583641	40.418868
3260.976592	324865.526596	40.423885
3264.230409	325359.700706	40.428903
3266.789255	325864.050055	40.433920
3269.884634	326374.449840	40.438938
3272.692285	326881.310466	40.443956
3275.826677	327400.825239	40.448973
3279.452362	327927.386258	40.453991
3282.605883	328455.815158	40.459008
3285.637409	328988.340728	40.464026
3288.598970	329527.846921	40.469044
3291.694581	330069.785754	40.474061
3295.153017	330615.770531	40.479079
3298.635644	331163.063083	40.484096
3301.798651	331717.500994	40.489114
3305.207236	332286.149972	40.494132
3308.220915	332845.516351	40.499149
3311.870007	333402.999856	40.504167
3314.917174	333969.523609	40.509184
3318.355329	334545.592200	40.514202
3321.587829	335129.547669	40.519220
3324.580503	335707.088200	40.524237
3328.178950	336288.203545	40.529255
3331.684618	336879.318247	40.534272
3335.174280	337468.650329	40.539290
3338.172189	338055.284627	40.544308
3341.476092	338655.406446	40.549325
3345.445620	339238.674417	40.554343
3348.770340	339840.903789	40.559360
3352.437134	340430.616425	40.564378
3355.995694	341025.560837	40.569396
3359.546477	341607.485537	40.574413
3362.570693	342196.203451	40.579431
3366.929849	342782.243645	40.584448
3370.196576	343375.063196	40.589466
3373.677460	343973.773654	40.594484
3377.162030	344557.409156	40.599501
3380.592439	345151.187050	40.604519
3383.872622	345743.659286	40.609536
3387.278025	346330.269137	40.614554
3390.705686	346923.813539	40.619572
3394.383180	347523.293055	40.624589
3397.663993	348121.936025	40.629607
3401.166905	348710.644388	40.634624
3404.423572	349315.177772	40.639642
3407.584041	349904.273118	40.644660
3411.233630	350507.125973	40.649677
3414.619956	351105.013662	40.654695
3418.256929	351704.651516	40.659712
3421.377700	352305.727690	40.664730
3424.876047	352904.426666	40.669748
3428.353965	353506.692432	40.674765
3432.175004	354103.315775	40.679783
3435.915441	354707.267258	40.684800
3438.958252	355302.112989	40.689818
3442.386142	355908.346361	40.694836
3445.943956	356507.221330	40.699853
3449.449280	357106.777390	40.704871
3453.073955	357705.339962	40.709888
3456.562244	358315.724965	40.714906
3459.918251	358900.997593	40.719924
3463.007866	359508.302915	40.724941
3466.817423	360100.528776	40.729959
3469.945801	360712.341228	40.734976
3473.365667	361313.095321	40.739994
3476.625185	361918.728838	40.745012
3480.206176	362515.542279	40.750016
3483.596351	363071.149184	40.755021
3486.910762	363587.296018	40.760026
3490.029936	364056.837952	40.765031
3493.020891	364471.381774	40.770036
3495.720361	364850.265842	40.775040
3498.353824	365168.378314	40.780045
3500.865425	365454.517366	40.785050
3502.786273	365679.512303	40.790055
3505.268431	365871.921544	40.795060
3506.628145	366035.005855	40.800064
3508.600422	366153.759348	40.805069
3510.270166	366234.422772	40.810074
3511.305883	366283.679382	40.815079
3512.576295	366302.537491	40.820084
3513.607564	366290.893042	40.825088
3514.370075	366263.461548	40.830093
3515.455798	366204.017062	40.835098
3515.783739	366132.850432	40.840103
3516.814325	366037.945148	40.845108
3516.919575	365934.773574	40.850112
3517.409399	365806.032278	40.855117
3518.042365	365674.651112	40.860122
3517.851324	365526.958521	40.865127
3518.129510	365366.792926	40.870132
3518.285382	365210.380523	40.875136
3518.123043	365042.811627	40.880141
3518.201100	364870.097211	40.885146
3517.947419	364691.462316	40.890151
3518.314780	364494.333555	40.895156
3518.082530	364312.110338	40.900160
3518.231513	364123.220234	40.905165
3518.286899	363921.664131	40.910170
3518.039400	363726.302927	40.915175
3518.563530	363525.458872	40.920180
3517.896220	363331.888256	40.925184
3517.453841	363130.937820	40.930189
3517.367220	362939.357910	40.935194
3517.453009	362731.106026	40.940199
3517.470378	362528.784030	40.945204
3516.789662	362332.362971	40.950208
3516.531286	362129.090142	40.955213
3516.700373	361932.280096	40.960218
3516.439195	361735.484886	40.965223
3516.016647	361529.794032	40.970228
3515.549846	361344.539690	40.975232
3515.654735	361155.688401	40.980237
3515.680017	360961.105190	40.985242
3515.054124	360775.490915	40.990247
3515.158970	360595.454154	40.995252
3514.649429	360411.903348	41.000256
3514.539251	360229.915691	41.005261
3514.384333	360053.626374	41.010266
3514.199856	359877.111914	41.015271
3513.895142	359695.837472	41.020276
3513.484099	359529.114881	41.025280
3513.444850	359351.888612	41.030285
3513.149324	359200.241803	41.035290
3512.793901	359033.990702	41.040295
3513.265017	358872.819907	41.045300
3512.750107	358716.604935	41.050304
3512.672447	358555.111239	41.055309
3512.431223	358404.824393	41.060314
3511.899830	358239.689170	41.065319
3511.837040	358084.239292	41.070324
3511.512530	357951.295842	41.075328
3511.546928	357796.083530	41.080333
3511.583756	357664.810814	41.085338
3511.255441	357509.805993	41.090343
3511.358057	357364.772283	41.095348
3510.649742	357225.353760	41.100352
3510.646458	357093.144496	41.105357
3510.322304	356963.856538	41.110362
3510.105523	356831.018580	41.115367
3510.093288	356700.130640	41.120372
3509.677789	356585.977599	41.125376
3509.993150	356447.438325	41.130381
3509.752260	356320.930473	41.135386
3509.714599	356215.587427	41.140391
3509.377765	356088.102337	41.145396
3509.369769	355973.171988	41.150400
3509.202129	355854.631529	41.155405
3509.330076	355723.514346	41.160410
3508.837970	355614.224200	41.165415
3508.943989	355512.999315	41.170420
3508.514897	355405.096546	41.175424
3508.854053	355287.034243	41.180429
3508.621895	355173.610015	41.185434
3508.584474	355080.005689	41.190439
3508.734123	354974.425988	41.195444
3508.101528	354869.476002	41.200448
3508.356107	354759.990440	41.205453
3508.300549	354652.916565	41.210458
3507.841745	354554.699477	41.215463
3508.075869	354448.596525	41.220468
3508.041525	354356.692542	41.225472
3508.250374	354260.124450	41.230477
3507.464442	354156.415999	41.235482
3507.288988	354063.109734	41.240487
3507.659050	353958.280291	41.245492
3507.596804	353871.564477	41.250496
3507.372672	353781.365941	41.255501
3507.247923	353700.098828	41.260506
3507.048605	353603.033058	41.265511
3507.218079	353509.290220	41.270516
3506.927593	353432.242213	41.275520
3506.859536	353340.569301	41.280525
3507.534306	353249.415991	41.285530
3506.718011	353166.297915	41.290535
3506.824910	353081.637943	41.295540
3506.614439	353007.753774	41.300544
3506.722881	352907.791117	41.305549
3506.779148	352823.163759	41.310554
3506.520341	352741.228761	41.315559
3506.569203	352656.576697	41.320564
3506.397032	352585.507086	41.325568
3506.074533	352507.038371	41.330573
3506.079343	352426.713781	41.335578
3506.067731	352358.287680	41.340583
3506.165069	352284.023495	41.345588
3506.253128	352209.989356	41.350592
3506.361791	352128.783608	41.355597
3506.200767	352056.363871	41.360602
3506.101268	351983.070139	41.365607
3506.363936	351900.162170	41.370612
3506.002321	351835.348146	41.375616
3506.060428	351754.022225	41.380621
3506.194561	351679.471308	41.385626
3506.087110	351615.100263	41.390631
3505.675485	351524.644938	41.395636
3505.822450	351460.208575	41.400640
3505.988722	351383.338774	41.405645
3505.517716	351312.160339	41.410650
3505.630518	351255.837837	41.415655
3505.371733	351174.737713	41.420660
3505.315443	351124.109959	41.425664
3505.389209	351045.499768	41.430669
3505.083263	350975.820117	41.435674
3505.262718	350923.198011	41.440679
3505.227113	350850.400177	41.445684
3504.899212	350800.195489	41.450688
3505.223253	350743.762967	41.455693
3504.993235	350679.307458	41.460698
3504.930113	350624.892350	41.465703
3505.084064	350563.935725	41.470708
3504.877805	350507.814101	41.475712
3504.660358	350439.161773	41.480717
3505.076476	350388.815251	41.485722
3504.700563	350341.261072	41.490727
3505.213045	350267.486925	41.495732
3504.885873	350219.314886	41.500736
3505.184140	350151.598532	41.505741
3505.155788	350084.365019	41.510746
3504.955313	350027.148573	41.515751
3504.843606	349971.290945	41.520756
3504.723591	349922.450709	41.525760
3504.760995	349858.968808	41.530765
3504.689650	349802.672454	41.535770
3504.939891	349745.487063	41.540775
3504.957048	349683.228187	41.545780
3504.615081	349627.126172	41.550784
3504.521999	349566.307817	41.555789
3504.346134	349518.339995	41.560794
3504.163346	349472.000145	41.565799
3504.306554	349418.567779	41.570804
3504.333145	349372.347736	41.575808
3504.354412	349318.451176	41.580813
3504.685969	349263.565648	41.585818
3504.413863	349210.858532	41.590823
3504.733765	349155.720422	41.595828
3504.401901	349110.826872	41.600832
3504.529235	349052.490010	41.605837
3504.705522	349002.712543	41.610842
3504.605530	348956.587880	41.615847
3504.656182	348893.661336	41.620852
3504.371092	348841.616617	41.625856
3504.565549	348786.039819	41.630861
3504.454692	348724.993883	41.635866
3504.508428	348675.972231	41.640871
3504.826750	348623.121456	41.645876
3504.357543	348569.299998	41.650880
3504.593401	348510.335165	41.655885
3504.727047	348454.207988	41.660890
3504.474960	348400.733802	41.665895
3504.655382	348351.412312	41.670900
3504.449815	348305.252327	41.675904
3504.440856	348242.867691	41.680909
3504.132401	348200.028468	41.685914
3504.487758	348154.264010	41.690919
3504.131262	348097.551522	41.695924
3504.512886	348042.884984	41.700928
3504.793922	347986.937463	41.705933
3504.231657	347935.976777	41.710938
3504.106289	347891.735850	41.715943
3504.518861	347838.004795	41.720948
3504.105239	347789.079984	41.725952
3504.461957	347732.738920	41.730957
3504.289029	347691.988035	41.735962
3504.375260	347645.171583	41.740967
3504.328566	347584.952521	41.745972
3504.468110	347532.737983	41.750976
3504.162249	347487.329734	41.755981
3504.142475	347428.250229	41.760986
3504.188080	347393.744432	41.765991
3504.054720	347334.072285	41.770996
3504.007453	347293.326783	41.776000
3503.802354	347247.978798	41.781005
3504.001480	347202.262773	41.786010
3504.050454	347158.400515	41.791015
3504.266192	347103.020985	41.796020
3504.429927	347050.420585	41.801024
3504.283509	347000.283573	41.806029
3504.264034	346960.677387	41.811034
3504.374312	346907.652887	41.816039
3504.162246	346854.424230	41.821044
3503.893316	346810.204213	41.826048
3504.218826	346757.806991	41.831053
3504.258019	346713.437207	41.836058
3503.923216	346667.447612	41.841063
3504.103825	346611.640541	41.846068
3503.914613	346576.407739	41.851072
3503.789570	346521.919260	41.856077
3504.012534	346477.393449	41.861082
3503.483381	346433.518515	41.866087
3503.658770	346386.406775	41.871092
3503.642458	346356.180728	41.876096
3503.644785	346310.494117	41.881101
3503.732042	346263.370495	41.886106
3503.433807	346236.747543	41.891111
3504.045506	346184.432016	41.896116
3503.782424	346136.371204	41.901120
3503.712489	346092.093856	41.906125
3503.799313	346051.071745	41.911130
3503.408406	346014.318882	41.916135
3503.791846	345958.631714	41.921140
3503.832787	345928.218408	41.926144
3503.980753	345879.228850	41.931149
3503.602942	345840.719499	41.936154
3503.606090	345800.371133	41.941159
3504.049811	345755.021872	41.946164
3503.926597	345712.582859	41.951168
3503.819114	345666.607376	41.956173
3503.931675	345626.470596	41.961178
3503.624465	345585.509239	41.966183
3504.166071	345537.246085	41.971188
3503.941494	345495.076817	41.976192
3503.744199	345438.487616	41.981197
3504.004063	345396.954725	41.986202
3503.772200	345358.015324	41.991207
3503.833445	345308.809619	41.996212
3503.680215	345274.917362	42.001216
3503.555693	345235.096683	42.006221
3504.050447	345185.416548	42.011226
3503.711189	345138.739106	42.016231
3503.815684	345094.662136	42.021236
3503.410257	345053.791697	42.026240
3503.457744	345018.139072	42.031245
3503.931679	344970.826363	42.036250
3503.873930	344924.867565	42.041255
3503.425422	344876.782977	42.046260
3503.550391	344841.499483	42.051264
3503.430228	344803.431937	42.056269
3503.641941	344756.973333	42.061274
3503.457565	344720.797131	42.066279
3503.273068	344677.883292	42.071284
3503.083883	344647.835179	42.076288
3503.536729	344594.702908	42.081293
3503.560034	344561.163848	42.086298
3503.357648	344532.210965	42.091303
3503.704518	344485.959788	42.096308
3503.538162	344463.484644	42.101312
3503.396289	344415.605943	42.106317
3503.562294	344368.060643	42.111322
3503.683115	344334.963841	42.116327
3503.819877	344285.694063	42.121332
3503.670753	344248.825395	42.126336
3503.544482	344210.758141	42.131341
3503.808257	344163.146494	42.136346
3503.489111	344121.625881	42.141351
3503.767726	344080.113901	42.146356
3503.683532	344035.556425	42.151360
3503.758444	343996.542311	42.156365
3503.434080	343950.623697	42.161370
3503.825228	343912.679001	42.166375
3503.644507	343862.212170	42.171380
3503.608027	343827.817228	42.176384
3503.418650	343786.809956	42.181389
3503.865691	343740.923576	42.186394
3503.369679	343712.803890	42.191399
3503.664996	343661.449066	42.196404
3503.600654	343621.693427	42.201408
3503.426787	343579.335930	42.206413
3503.943784	343541.015281	42.211418
3503.447373	343493.622708	42.216423
3503.567754	343457.041791	42.221428
3503.662772	343417.083137	42.226432
3503.489417	343379.810496	42.231437
3503.576399	343334.106736	42.236442
3503.400823	343304.767260	42.241447
3503.483049	343249.376826	42.246452
3503.358057	343215.732404	42.251456
3503.251164	343179.923917	42.256461
3503.688425	343144.869777	42.261466
3503.179276	343101.140007	42.266471
3503.806910	343048.359551	42.271476
3503.262659	343018.111008	42.276480
3503.631980	342978.439704	42.281485
3503.770462	342931.837483	42.286490
3503.175087	342892.138216	42.291495
3503.453341	342853.091172	42.296500
3503.473845	342826.899068	42.301504
3503.418609	342785.513768	42.306509
3503.518655	342750.333721	42.311514
3503.369737	342710.437640	42.316519
3503.506908	342669.073113	42.321524
3503.178773	342636.807344	42.326528
3503.436406	342590.135271	42.331533
3503.422954	342548.082098	42.336538
3502.953130	342518.202935	42.341543
3503.342181	342476.595572	42.346548
3503.441833	342439.584558	42.351552
3503.181854	342411.503366	42.356557
3503.368364	342365.706567	42.361562
3503.108082	342332.997705	42.366567
3503.066901	342294.915105	42.371572
3503.205308	342262.423829	42.376576
3503.002774	342225.917295	42.381581
3503.176836	342183.198833	42.386586
3503.105063	342151.324977	42.391591
3503.310154	342107.635375	42.396596
3503.333213	342084.188418	42.401600
3502.888120	342051.101220	42.406605
3503.072752	342009.931943	42.411610
3503.260372	341987.222121	42.416615
3503.327646	341945.155660	42.421620
3503.167664	341923.898372	42.426624
3503.000722	341877.291417	42.431629
3503.238845	341830.367098	42.436634
3503.353767	341809.066961	42.441639
3503.451008	341777.751288	42.446644
3503.156759	341737.927567	42.451648
3503.011393	341697.038119	42.456653
3503.293674	341665.642697	42.461658
3503.097766	341627.227469	42.466663
3503.377516	341584.313841	42.471668
3503.103728	341553.309977	42.476672
3502.935958	341518.831478	42.481677
3503.062642	341487.968656	42.486682
3502.847450	341450.598755	42.491687
3503.016059	341418.788537	42.496692
3503.066240	341390.836254	42.501696
3503.151306	341357.691330	42.506701
3503.064314	341317.860309	42.511706
3503.008724	341291.144922	42.516711
3503.057224	341243.867917	42.521716
3503.082879	341223.954401	42.526720
3502.844193	341182.087205	42.531725
3503.222977	341143.556592	42.536730
3502.982862	341106.291915	42.541735
3503.052489	341078.717772	42.546740
3502.878824	341040.323871	42.551744
3502.855415	341006.839511	42.556749
3503.086804	340974.256294	42.561754
3503.408318	340945.549460	42.566759
3503.175481	340911.182202	42.571764
3502.937928	340878.392165	42.576768
3503.025376	340838.736880	42.581773
3503.440377	340808.057449	42.586778
3503.025726	340783.024931	42.591783
3503.178834	340746.436091	42.596788
3502.896957	340711.542286	42.601792
3503.157387	340675.852075	42.606797
3503.260314	340639.270933	42.611802
3502.913175	340601.386681	42.616807
3503.019359	340569.636269	42.621812
3503.248938	340539.799155	42.626816
3502.911080	340507.787223	42.631821
3503.202265	340459.454285	42.636826
3503.188666	340435.147382	42.641831
3503.078545	340389.216179	42.646836
3503.168972	340366.291587	42.651840
3503.037867	340328.297141	42.656845
3503.359239	340285.909454	42.661850
3503.232891	340247.125907	42.666855
3503.253106	340213.659438	42.671860
3502.824672	340185.653542	42.676864
3502.789480	340146.067424	42.681869
3502.961028	340114.484433	42.686874
3502.415734	340084.589520	42.691879
3503.257693	340054.300708	42.696884
3502.870225	340029.009145	42.701888
3503.028778	339990.257270	42.706893
3503.176832	339954.176969	42.711898
3503.033676	339927.194469	42.716903
3502.949950	339891.302743	42.721908
3502.858021	339863.091657	42.726912
3502.572314	339832.367854	42.731917
3503.237821	339805.055995	42.736922
3502.733637	339775.840995	42.741927
3503.217470	339741.005082	42.746932
3502.955055	339709.946978	42.751936
3502.875322	339668.688976	42.756941
3503.073179	339636.847183	42.761946
3503.079646	339602.949994	42.766951
3502.786682	339573.651102	42.771956
3503.076004	339541.260989	42.776960
3503.140831	339516.305538	42.781965
3502.903624	339477.589264	42.786970
3502.733648	339448.398275	42.791975
3502.734627	339409.772006	42.796980
3503.010577	339380.562428	42.801985
3502.970761	339353.715987	42.806989
3502.938284	339315.679686	42.811994
3503.003552	339272.389784	42.816999
3503.153058	339242.131756	42.822004
3502.870158	339221.502268	42.827009
3503.030438	339187.148460	42.832013
3502.948479	339152.959458	42.837018
3502.877640	339122.710189	42.842023
3502.808639	339079.186658	42.847028
3502.803091	339050.122332	42.852033
3502.779991	339024.747928	42.857037
3503.206819	338990.479599	42.862042
3502.718525	338967.008439	42.867047
3503.027761	338939.293641	42.872052
3503.230312	338906.789313	42.877057
3502.888602	338868.520939	42.882061
3502.876089	338842.915897	42.887066
3502.858411	338802.333831	42.892071
3503.400774	338771.734553	42.897076
3502.864686	338742.625391	42.902081
3502.874543	338711.549483	42.907085
3503.150849	338665.047348	42.912090
3502.641707	338648.368853	42.917095
3502.807792	338609.385452	42.922100
3502.661319	338583.801072	42.927105
3502.301079	338551.180566	42.932109
3502.651566	338532.588190	42.937114
3502.638905	338508.152687	42.942119
3502.555054	338469.894623	42.947124
3502.951183	338438.554935	42.952129
3502.573740	338415.905339	42.957133
3502.696376	338380.920883	42.962138
3502.584298	338358.102809	42.967143
3502.899665	338324.232636	42.972148
3502.791613	338281.146521	42.977153
3502.951691	338258.540329	42.982157
3502.672624	338231.119972	42.987162
3502.746104	338212.417960	42.992167
3502.623909	338177.547695	42.997172
3502.719048	338152.179709	43.002177
3502.836856	338125.104387	43.007181
3502.838966	338089.451804	43.012186
3502.463753	338063.216048	43.017191
3502.830597	338026.743753	43.022196
3502.945820	338003.966374	43.027201
3502.591761	337970.327191	43.032205
3502.776094	337941.969891	43.037210
3502.649502	337922.001941	43.042215
3502.854228	337882.528578	43.047220
3502.756898	337857.266626	43.052225
3502.414424	337819.658438	43.057229
3502.690458	337789.404935	43.062234
3502.617429	337779.244526	43.067239
3502.564154	337750.517172	43.072244
3502.622591	337717.398454	43.077249
3502.376536	337685.039129	43.082253
3502.753852	337648.564826	43.087258
3502.475024	337631.137980	43.092263
3502.692386	337596.061737	43.097268
3502.816881	337577.427750	43.102273
3502.601481	337543.970036	43.107277
3503.012529	337516.823200	43.112282
3502.484865	337493.560650	43.117287
3502.532651	337460.799379	43.122292
3502.457111	337429.481359	43.127297
3502.395734	337413.470091	43.132301
3502.711574	337382.141988	43.137306
3502.711420	337353.634927	43.142311
3502.696389	337321.722504	43.147316
3502.645874	337304.056531	43.152321
3502.829030	337271.070581	43.157325
3502.533774	337239.379705	43.162330
3502.681954	337224.861564	43.167335
3502.945742	337191.176376	43.172340
3502.673715	337154.039715	43.177345
3502.832232	337124.083682	43.182349
3502.982728	337099.698135	43.187354
3502.527250	337069.939325	43.192359
3502.766351	337040.250419	43.197364
3502.465543	337015.299282	43.202369
3502.755807	336987.128200	43.207373
3503.114789	336948.926779	43.212378
3502.573026	336926.810435	43.217383
3502.632724	336899.895830	43.222388
3502.790609	336872.075857	43.227393
3502.754578	336839.403364	43.232397
3502.736037	336800.548479	43.237402
3502.623072	336788.232405	43.242407
3502.408735	336745.669627	43.247412
3502.513537	336720.171989	43.252417
3502.671605	336701.583193	43.257421
3503.056609	336670.676042	43.262426
3502.694692	336644.030304	43.267431
3502.768000	336607.347965	43.272436
3502.923081	336575.535574	43.277441
3502.477472	336542.621383	43.282445
3502.703251	336509.907856	43.287450
3502.654850	336491.503668	43.292455
3502.498934	336460.375344	43.297460
3502.663733	336443.158636	43.302465
3502.243770	336402.585636	43.307469
3502.494526	336384.490875	43.312474
3502.452267	336370.383495	43.317479
3502.505163	336337.874734	43.322484
3502.770020	336299.432977	43.327489
3502.480319	336281.066233	43.332493
3502.562378	336246.950702	43.337498
3501.911286	336238.431111	43.342503
3502.329769	336204.263189	43.347508
3502.538214	336180.910687	43.352513
3502.408672	336155.499987	43.357517
3502.649677	336121.130727	43.362522
3502.707343	336101.768888	43.367527
3501.998393	336070.217672	43.372532
3502.200767	336058.132025	43.377537
3502.214517	336033.232997	43.382541
3502.575080	336001.464429	43.387546
3502.207167	335982.448497	43.392551
3502.534025	335952.643333	43.397556
3502.533714	335942.776274	43.402561
3502.345305	335912.059442	43.407565
3502.753431	335891.625709	43.412570
3502.460360	335852.075038	43.417575
3502.616021	335823.466250	43.422580
3502.871880	335798.656545	43.427585
3502.425255	335767.776325	43.432589
3502.705834	335740.648483	43.437594
3502.245170	335721.265379	43.442599
3502.827435	335692.005184	43.447604
3502.619410	335668.233971	43.452609
3502.074658	335637.267186	43.457613
3502.474850	335613.503017	43.462618
3502.610632	335590.619217	43.467623
3502.633575	335563.912809	43.472628
3502.526985	335539.718825	43.477633
3502.308474	335507.251570	43.482637
3502.724512	335488.444000	43.487642
3502.447934	335463.030274	43.492647
3502.719015	335435.700235	43.497652
3502.778430	335405.859956	43.502657
3502.279945	335372.240865	43.507661
3502.352271	335347.993483	43.512666
3502.319214	335333.807981	43.517671
3502.657447	335299.575419	43.522676
3502.599152	335278.272959	43.527681
3502.198445	335249.801170	43.532685
3502.555443	335226.908154	43.537690
3502.245277	335206.712979	43.542695
3502.300932	335171.303549	43.547700
3502.225981	335158.879290	43.552705
3502.241605	335128.486104	43.557709
3502.563482	335106.895500	43.562714
3502.305324	335084.784781	43.567719
3502.065814	335060.280556	43.572724
3502.129812	335033.491083	43.577729
3502.351455	335016.900665	43.582733
3502.743145	334991.814967	43.587738
3502.432409	334970.144704	43.592743
3502.375742	334942.967033	43.597748
3502.397701	334922.592861	43.602753
3502.230948	334893.067116	43.607757
3502.334734	334866.983427	43.612762
3502.425664	334850.031796	43.617767
3502.341071	334808.896223	43.622772
3502.493037	334797.275788	43.627777
3502.262844	334772.464740	43.632781
3502.539983	334745.234981	43.637786
3502.466100	334730.674122	43.642791
3502.250567	334698.358290	43.647796
3502.610457	334676.659794	43.652801
3502.146730	334649.443525	43.657805
3502.395552	334626.490679	43.662810
3502.676463	334604.804432	43.667815
3502.401497	334575.295276	43.672820
3502.552312	334547.652684	43.677825
3502.705634	334521.103267	43.682829
3502.734187	334491.902864	43.687834
3502.338204	334466.201853	43.692839
3502.280376	334440.473634	43.697844
3502.453394	334435.614786	43.702849
3502.575169	334405.840301	43.707853
3502.490670	334365.390897	43.712858
3502.208110	334344.962069	43.717863
3502.167167	334312.517006	43.722868
3502.388711	334299.613973	43.727873
3502.502363	334272.994256	43.732877
3502.508492	334248.502139	43.737882
3502.505903	334234.464072	43.742887
3502.749818	334202.127181	43.747892
3502.758950	334177.736280	43.752897
3502.659196	334149.471145	43.757901
3502.631702	334119.795958	43.762906
3502.521160	334098.272064	43.767911
3502.706515	334066.122195	43.772916
3502.712090	334038.374668	43.777921
3502.275266	334008.839389	43.782925
3502.751367	333976.364442	43.787930
3502.442337	333960.008732	43.792935
3502.568100	333924.002265	43.797940
3502.907771	333900.856811	43.802945
3502.551543	333871.563208	43.807949
3502.619155	333846.272850	43.812954
3502.338067	333819.409048	43.817959
3502.598846	333787.374368	43.822964
3502.563387	333761.413310	43.827969
3502.530297	333745.548653	43.832973
3502.735577	333709.326147	43.837978
3502.432034	333677.633517	43.842983
3502.285192	333654.538187	43.847988
3502.277641	333632.972567	43.852993
3502.299206	333610.766584	43.857997
3502.338585	333588.710413	43.863002
3501.938719	333577.760429	43.868007
3502.120146	333545.610728	43.873012
3502.184855	333522.634995	43.878017
3501.917302	333511.460938	43.883021
3502.568768	333474.685550	43.888026
3502.142063	333454.583863	43.893031
3502.172180	333436.216816	43.898036
3502.536149	333414.211765	43.903041
3502.391028	333388.547278	43.908045
3502.382314	333359.707859	43.913050
3502.217413	333347.424162	43.918055
3502.047954	333320.695231	43.923060
3502.275313	333299.652392	43.928065
3502.165819	333288.250210	43.933069
3502.382561	333255.280911	43.938074
3502.245009	333234.549152	43.943079
3502.111783	333208.653794	43.948084
3502.387800	333191.520017	43.953089
3502.406111	333170.585936	43.958093
3502.373306	333138.443795	43.963098
3502.482063	333107.652987	43.968103
3502.285439	333087.260970	43.973108
3502.870603	333060.923091	43.978113
3502.734422	333042.683464	43.983117
3502.258703	333005.421763	43.988122
3502.319129	332983.158499	43.993127
3502.053433	332970.890365	43.998132
3502.459783	332947.021823	44.003137
3502.372218	332929.283241	44.008141
3502.557306	332897.666520	44.013146
3502.185246	332877.352557	44.018151
3502.257734	332851.908178	44.023156
3502.645255	332822.065659	44.028161
3502.236907	332800.155001	44.033165
3501.919550	332772.533099	44.038170
3502.178726	332755.045679	44.043175
3502.413533	332732.195598	44.048180
3502.479572	332710.923203	44.053185
3502.379069	332695.500965	44.058189
3502.283606	332659.527724	44.063194
3502.591111	332641.371462	44.068199
3502.647614	332619.973333	44.073204
3502.675729	332584.667494	44.078209
3502.086340	332566.192962	44.083213
3502.310254	332532.840419	44.088218
3502.425887	332515.349793	44.093223
3502.385933	332491.397816	44.098228
3502.389103	332459.732740	44.103233
3502.519499	332443.257127	44.108237
3502.545149	332407.646305	44.113242
3502.218951	332391.597792	44.118247
3502.093644	332365.573460	44.123252
3502.511243	332346.255413	44.128257
3502.452749	332314.879583	44.133261
3502.144389	332290.206237	44.138266
3502.321375	332277.411186	44.143271
3502.199890	332248.105233	44.148276
3502.407805	332235.407090	44.153281
3501.880374	332216.058000	44.158285
3502.228979	332188.128572	44.163290
3502.088828	332162.996594	44.168295
3502.326296	332149.657980	44.173300
3502.038616	332128.999848	44.178305
3501.984265	332111.153982	44.183309
3502.266443	332086.057969	44.188314
3502.170177	332070.889158	44.193319
3502.404944	332042.010853	44.198324
3502.607589	332016.291325	44.203329
3502.198786	332001.400025	44.208333
3502.378530	331976.981162	44.213338
3502.605970	331951.410335	44.218343
3502.283830	331924.627883	44.223348
3502.550508	331888.648431	44.228353
3502.118993	331865.952389	44.233357
3502.594782	331847.184583	44.238362
3502.475508	331821.311547	44.243367
3502.566304	331786.300426	44.248372
3502.667770	331757.875030	44.253377
3501.929712	331752.267424	44.258381
3502.251059	331716.024963	44.263386
3502.170399	331701.057050	44.268391
3502.343166	331674.884129	44.273396
3502.290659	331653.349820	44.278401
3502.268841	331629.775993	44.283405
3502.254663	331612.737536	44.288410
3502.376930	331595.067420	44.293415
3501.926509	331571.789161	44.298420
3502.261380	331540.783867	44.303425
3502.314836	331523.734846	44.308429
3502.447699	331499.704488	44.313434
3502.255811	331484.677497	44.318439
3502.198255	331450.553920	44.323444
3502.210233	331430.942454	44.328449
3502.147764	331405.772458	44.333453
3502.343573	331386.742785	44.338458
3502.464543	331371.667065	44.343463
3502.205136	331342.458187	44.348468
3502.546572	331318.395260	44.353473
3502.357972	331298.535161	44.358477
3502.534901	331267.528792	44.363482
3502.405181	331250.330114	44.368487
3502.202352	331217.042837	44.373492
3502.726672	331202.438406	44.378497
3502.605286	331169.443628	44.383501
3502.428617	331137.067850	44.388506
3502.255084	331122.851764	44.393511
3502.442531	331090.877106	44.398516
3502.215639	331062.960116	44.403521
3502.089994	331035.866688	44.408525
3502.234551	331020.736292	44.413530
3502.565589	331001.761690	44.418535
3502.104162	330979.553037	44.423540
3502.245031	330957.835640	44.428545
3501.850963	330934.421054	44.433549
3502.568583	330914.546912	44.438554
3502.179146	330887.977688	44.443559
3502.294693	330871.529148	44.448564
3502.335588	330841.204906	44.453569
3502.274592	330820.943186	44.458573
3502.388157	330791.879330	44.463578
3502.121781	330765.265437	44.468583
3502.162232	330747.175275	44.473588
3501.958940	330730.521944	44.478593
3501.646950	330700.023592	44.483597
3501.944962	330688.633527	44.488602
3501.474914	330672.326898	44.493607
3501.657894	330657.139512	44.498612
3501.688063	330647.393504	44.503617
3502.145902	330627.000076	44.508621
3502.111234	330608.183930	44.513626
3502.123971	330588.800833	44.518631
3502.009347	330580.679734	44.523636
3502.309722	330549.729885	44.528641
3502.260296	330536.867752	44.533645
3502.636419	330512.366535	44.538650
3502.405623	330489.638450	44.543655
3501.874818	330458.716132	44.548660
3502.245644	330435.207652	44.553665
3501.814000	330414.520134	44.558669
3502.193040	330402.506938	44.563674
3502.290390	330380.567078	44.568679
3502.236238	330364.068426	44.573684
3502.091129	330323.547872	44.578689
3501.879444	330321.062952	44.583693
3502.085997	330291.017723	44.588698
3501.869918	330281.615164	44.593703
3501.754656	330257.317428	44.598708
3501.951984	330242.229387	44.603713
3501.860905	330235.885004	44.608717
3502.325078	330214.167753	44.613722
3501.945380	330192.556371	44.618727
3501.982019	330168.997995	44.623732
3502.263693	330154.507237	44.628737
3501.728866	330142.102034	44.633741
3502.516246	330116.213947	44.638746
3502.304007	330090.405092	44.643751
3501.889390	330066.204691	44.648756
3502.240127	330041.859741	44.653761
3502.113680	330021.607790	44.658765
3502.001951	329998.097833	44.663770
3501.936509	329984.983658	44.668775
3501.746383	329970.795167	44.673780
3502.240100	329949.327524	44.678785
3502.282194	329931.440210	44.683789
3502.569847	329899.754205	44.688794
3501.945024	329885.836809	44.693799
3501.554046	329864.099825	44.698804
3502.162317	329851.745567	44.703809
3502.184008	329834.522701	44.708813
3502.065368	329803.891819	44.713818
3502.041412	329781.105698	44.718823
3502.234636	329763.754367	44.723828
3502.131853	329743.295106	44.728833
3501.751275	329731.298170	44.733837
3502.088858	329698.357900	44.738842
3501.871856	329689.057083	44.743847
3502.405246	329677.248565	44.748852
3502.142515	329647.708271	44.753857
3501.942304	329642.347319	44.758861
3501.753223	329614.728631	44.763866
3501.735645	329603.616280	44.768871
3501.962193	329585.064218	44.773876
3502.030929	329555.777499	44.778881
3502.005957	329541.130749	44.783885
3501.842324	329519.332760	44.788890
3502.092011	329512.095860	44.793895
3501.834206	329487.540038	44.798900
3502.177416	329473.014017	44.803905
3501.902883	329444.391085	44.808909
3501.923225	329423.759885	44.813914
3501.998355	329423.570347	44.818919
3502.492013	329400.474538	44.823924
3502.125380	329367.567269	44.828929
3501.867620	329349.904400	44.833933
3502.256337	329332.497022	44.838938
3501.997265	329311.349660	44.843943
3502.205914	329291.070621	44.848948
3502.116645	329273.254321	44.853953
3502.141518	329255.776349	44.858957
3501.975227	329230.570234	44.863962
3502.107792	329220.222916	44.868967
3501.850888	329190.376142	44.873972
3502.555286	329175.997293	44.878977
3502.287144	329152.918142	44.883981
3501.965487	329124.302310	44.888986
3502.192904	329104.885072	44.893991
3502.117993	329092.382530	44.898996
3501.898878	329058.510923	44.904001
3502.166003	329056.536437	44.909005
3502.341414	329016.346193	44.914010
3501.928450	329005.422379	44.919015
3501.818444	328985.447129	44.924020
3501.947404	328966.604732	44.929025
3501.377518	328959.749626	44.934029
3501.694085	328945.278429	44.939034
3501.854683	328932.968112	44.944039
3501.603344	328930.387530	44.949044
3502.126691	328900.266505	44.954049
3502.138425	328888.996775	44.959053
3502.278958	328860.970163	44.964058
3502.029911	328845.951049	44.969063
3502.161631	328821.588555	44.974068
3501.728364	328805.021063	44.979073
3502.084559	328798.555974	44.984077
3501.807027	328761.971554	44.989082
3502.088889	328749.718618	44.994087
3501.963117	328739.462247	44.999092
3501.928138	328716.906150	45.004097
3501.865167	328688.376927	45.009101
3501.979994	328671.622345	45.014106
3502.000490	328668.134619	45.019111
3502.008458	328646.945345	45.024116
3502.272160	328623.020040	45.029121
3502.093122	328597.128730	45.034125
3502.089008	328574.796673	45.039130
3501.901997	328562.235100	45.044135
3501.895287	328547.712320	45.049140
3501.997527	328522.972688	45.054145
3501.933189	328504.160152	45.059149
3501.843559	328486.190935	45.064154
3502.177356	328459.075103	45.069159
3502.000778	328449.208106	45.074164
3502.140519	328419.273591	45.079169
3501.725088	328413.284621	45.084173
3502.300348	328391.905189	45.089178
3501.763236	328378.838440	45.094183
3501.667801	328345.430265	45.099188
3502.093855	328329.263014	45.104193
3502.144327	328327.780059	45.109197
3502.328555	328293.514360	45.114202
3502.207096	328283.358945	45.119207
3502.042192	328264.104091	45.124212
3501.959062	328244.480393	45.129217
3501.732323	328221.496001	45.134221
3502.041927	328202.625131	45.139226
3502.075016	328180.058137	45.144231
3501.642587	328169.671284	45.149236
3502.264399	328158.153792	45.154241
3502.132413	328135.892261	45.159245
3502.227028	328110.695704	45.164250
3501.963071	328090.591342	45.169255
3501.909062	328071.191955	45.174260
3502.156832	328043.351570	45.179265
3502.013899	328032.512649	45.184269
3501.847508	328004.889305	45.189274
3501.912120	327991.703357	45.194279
3502.032056	327975.202051	45.199284
3502.044719	327950.730368	45.204289
3502.253128	327939.658692	45.209293
3502.322333	327903.324763	45.214298
3502.162242	327895.388240	45.219303
3501.972277	327873.898680	45.224308
3501.821755	327847.697205	45.229313
3501.959682	327830.989547	45.234317
3502.191091	327817.548657	45.239322
3501.781367	327790.548071	45.244327
3501.831553	327780.035142	45.249332
3501.934998	327760.738286	45.254337
3501.903438	327747.923335	45.259341
3502.235216	327716.991817	45.264346
3502.054212	327704.632532	45.269351
3501.756752	327693.944748	45.274356
3502.039758	327659.332457	45.279361
3501.905931	327652.968874	45.284365
3501.868017	327628.428554	45.289370
3502.029966	327616.906158	45.294375
3501.864317	327600.016714	45.299380
3502.036438	327576.003286	45.304385
3501.964211	327569.477482	45.309389
3502.192552	327547.337608	45.314394
3502.095733	327540.256018	45.319399
3501.725947	327510.171180	45.324404
3501.744457	327484.477335	45.329409
3501.905186	327481.501857	45.334413
3501.840846	327459.203984	45.339418
3501.894364	327444.645994	45.344423
3501.720084	327420.584629	45.349428
3502.126426	327404.572694	45.354433
3501.673941	327400.268169	45.359437
3502.009420	327370.658525	45.364442
3501.939716	327359.960647	45.369447
3501.511375	327342.272554	45.374452
3502.015059	327323.549128	45.379457
3502.054074	327314.436845	45.384461
3502.097394	327283.626191	45.389466
3502.229734	327277.221129	45.394471
3502.131129	327258.006346	45.399476
3502.329149	327228.443425	45.404481
3502.151109	327210.156711	45.409485
3502.173016	327183.775347	45.414490
3501.486729	327164.524786	45.419495
3501.757440	327152.756399	45.424500
3502.113905	327135.276771	45.429505
3502.244681	327118.035752	45.434509
3502.087679	327097.812498	45.439514
3502.408751	327077.820084	45.444519
3501.921545	327054.824679	45.449524
3502.405477	327032.848245	45.454529
3501.937422	327022.161391	45.459533
3502.293249	326991.123824	45.464538
3502.501485	326967.307910	45.469543
3502.249961	326952.008658	45.474548
3502.054185	326930.799305	45.479553
3501.987050	326914.962603	45.484557
3502.331224	326889.777319	45.489562
3502.347183	326876.166143	45.494567
3502.154975	326843.458578	45.499572
3502.230386	326820.019367	45.504577
3502.095929	326801.827434	45.509581
3502.017343	326776.606117	45.514586
3502.216938	326760.473476	45.519591
3501.938458	326735.384988	45.524596
3502.206910	326717.664503	45.529601
3501.927773	326706.108736	45.534605
3502.055726	326683.170015	45.539610
3501.864003	326655.600559	45.544615
3502.124561	326640.577625	45.549620
3502.200173	326613.246349	45.554625
3502.040941	326607.954922	45.559629
3502.240784	326586.963636	45.564634
3502.211932	326571.349778	45.569639
3501.854090	326548.791826	45.574644
3502.108045	326520.796800	45.579649
3502.058601	326503.609001	45.584653
3502.170787	326481.664679	45.589658
3502.168548	326456.456720	45.594663
3502.104021	326444.129795	45.599668
3502.048665	326413.461020	45.604673
3502.003668	326400.469669	45.609677
3502.166044	326381.112106	45.614682
3502.220466	326353.402390	45.619687
3502.007009	326330.033284	45.624692
3501.802350	326310.885429	45.629697
3501.731338	326306.292485	45.634701
3502.092622	326281.790975	45.639706
3501.881264	326274.294547	45.644711
3501.838829	326254.434607	45.649716
3501.992056	326249.883075	45.654721
3501.559507	326229.269826	45.659725
3501.793477	326206.339775	45.664730
3501.869040	326193.940100	45.669735
3501.782771	326175.358822	45.674740
3502.247066	326147.279933	45.679745
3501.950220	326138.855590	45.684749
3501.642218	326117.841338	45.689754
3501.679467	326107.024734	45.694759
3501.453642	326101.412913	45.699764
3501.859631	326075.632438	45.704769
3501.796563	326062.135037	45.709773
3501.917708	326049.321222	45.714778
3501.994093	326025.677898	45.719783
3501.813110	326017.642504	45.724788
3501.939237	325985.266273	45.729793
3501.851552	325979.989068	45.734797
3501.821335	325968.852235	45.739802
3501.621089	325952.221861	45.744807
3501.789820	325930.624572	45.749812
3501.680397	325908.612674	45.754817
3501.727283	325880.267863	45.759821
3501.667782	325817.751125	45.764826
3501.606698	325702.552625	45.769831
3500.887963	325565.833834	45.774836
3500.686916	325360.580050	45.779841
3499.895750	325147.963653	45.784845
3499.718122	324860.970474	45.789850
3498.914454	324553.823562	45.794855
3497.954892	324188.494543	45.799860
3496.745550	323790.461050	45.804865
3495.726175	323369.397006	45.809869
3494.738896	322905.966732	45.814874
3493.283656	322402.943297	45.819879
3491.788262	321866.822328	45.824884
3490.427108	321296.964894	45.829889
3488.498945	320702.408588	45.834893
3486.695162	320071.163738	45.839898
3485.419797	319418.812584	45.844903
3483.470499	318736.636604	45.849908
3481.719592	318013.711099	45.854913
3479.731654	317278.903352	45.859917
3477.361921	316513.763495	45.864922
3475.533008	315725.372560	45.869927
3473.080956	314908.618170	45.874932
3470.982458	314066.222200	45.879937
3468.186948	313225.471484	45.884941
3465.768733	312332.534117	45.889946
3463.090050	311434.531118	45.894951
3460.616405	310519.124640	45.899956
3458.524628	309581.604082	45.904961
3455.575672	308632.900090	45.909965
3452.838035	307658.594977	45.914970
3450.006285	306678.941230	45.919975
3447.178183	305673.767821	45.924980
3444.724546	304656.020561	45.929985
3441.456989	303636.674764	45.934989
3438.363702	302592.543967	45.939994
3435.425546	301532.232455	45.944999
3432.300021	300464.700943	45.950004
3429.023887	299392.336089	45.955009
3425.986076	298319.709772	45.960013
3422.605020	297223.674060	45.965018
3419.855388	296128.791732	45.970023
3416.547931	295013.154070	45.975028
3413.045469	293894.292896	45.980033
3409.901347	292782.813391	45.985037
3406.627685	291640.099814	45.990042
3403.291855	290508.473649	45.995047
3399.681438	289361.876044	46.000052
3396.243292	288218.871479	46.005057
3392.789380	287074.398306	46.010061
3389.545110	285915.438266	46.015066
3386.037948	284756.524800	46.020071
3382.362033	283600.393173	46.025076
3378.977165	282428.285403	46.030081
3375.538338	281264.823177	46.035085
3371.898378	280093.048468	46.040090
3368.723673	278919.604548	46.045095
3364.908861	277749.908641	46.050100
3361.374631	276572.920716	46.055105
3357.472371	275390.982388	46.060109
3354.448922	274216.401537	46.065114
3350.658964	273033.393789	46.070119
3346.734836	271852.962422	46.075124
3343.332917	270672.816001	46.080129
3339.729938	269492.125360	46.085133
3336.020663	268309.704816	46.090138
3332.939363	267129.565571	46.095143
3329.086752	265943.802837	46.100148
3325.344724	264744.538425	46.105153
3321.412390	263572.104136	46.110157
3318.390606	262385.942638	46.115162
3314.669453	261197.712816	46.120167
3310.416356	260006.523133	46.125172
3307.484425	258817.153210	46.130177
3303.492442	257634.965385	46.135181
3299.597564	256455.756542	46.140186
3295.715284	255255.016214	46.145191
3291.968846	254093.080852	46.150196
3288.976815	252898.192058	46.155201
3284.924819	251729.689700	46.160205
3281.043018	250546.101085	46.165210
3277.340831	249369.530465	46.170215
3273.763767	248199.120972	46.175220
3270.099930	247017.639022	46.180225
3266.123056	245857.540543	46.185229
3262.388401	244693.399277	46.190234
3258.736489	243520.808913	46.195239
3254.781250	242366.775157	46.200244
3251.463666	241196.897330	46.205249
3247.358665	240052.528888	46.210253
3244.106057	238889.813215	46.215258
3240.411331	237738.291780	46.220263
3236.099653	236590.402610	46.225268
3232.889636	235430.088023	46.230273
3228.880560	234276.007113	46.235277
3224.886800	233128.950454	46.240282
3221.391007	231990.804464	46.245287
3217.467804	230844.139955	46.250292
3213.997651	229700.332241	46.255297
3210.196772	228564.648412	46.260301
3206.368495	227433.399572	46.265306
3202.340505	226312.292500	46.270311
3198.400447	225195.857879	46.275316
3195.160745	224063.268928	46.280321
3191.278364	222945.068650	46.285325
3187.548662	221828.348140	46.290330
3183.918261	220716.172320	46.295335
3179.831847	219603.203040	46.300340
3176.344982	218489.149033	46.305345
3172.358368	217388.622552	46.310349
3168.872480	216276.406857	46.315354
3165.238801	215174.200764	46.320359
3161.156193	214086.737613	46.325364
3157.908344	212989.317068	46.330369
3153.680578	211904.201233	46.335373
3150.220562	210809.826764	46.340378
3146.237769	209717.677357	46.345383
3142.392271	208629.840851	46.350388
3138.874972	207551.203125	46.355393
3134.916280	206479.311859	46.360397
3131.220821	205397.605419	46.365402
3127.474701	204328.544637	46.370407
3123.795123	203258.944673	46.375412
3120.175225	202187.711806	46.380417
3116.073025	201129.370601	46.385421
3112.353909	200067.054610	46.390426
3109.086097	199028.868984	46.395431
3104.813965	197974.777222	46.400436
3101.546691	196928.838715	46.405441
3097.584713	195888.745946	46.410445
3094.078300	194849.405104	46.415450
3090.354977	193809.520470	46.420455
3086.429808	192775.558271	46.425460
3082.936606	191730.281742	46.430465
3079.353352	190696.334891	46.435469
3075.376806	189673.331976	46.440474
3071.557022	188652.172837	46.445479
3067.761947	187628.778442	46.450484
3064.116051	186602.340352	46.455489
3060.157728	185608.885994	46.460493
3056.318379	184584.866262	46.465498
3052.781247	183590.373227	46.470503
3048.871296	182592.969214	46.475508
3044.969401	181585.720278	46.480513
3041.208402	180603.286539	46.485517
3037.333481	179606.851390	46.490522
3033.684965	178624.370949	46.495527
3029.723989	177660.231889	46.500532
3026.275332	176674.419905	46.505537
3022.060708	175707.822016	46.510541
3018.870778	174740.184985	46.515546
3015.224728	173776.182390	46.520551
3011.100777	172830.699282	46.525556
3007.469536	171869.607738	46.530561
3003.712339	170919.482926	46.535565
2999.556750	169968.184725	46.540570
2995.764988	169036.178420	46.545575
2991.738820	168111.005410	46.550580
2988.116235	167175.178263	46.555585
2984.346553	166258.683769	46.560589
2980.230874	165341.606188	46.565594
2976.611610	164430.942703	46.570599
2972.668586	163533.541518	46.575604
2969.202976	162623.069962	46.580609
2965.241865	161727.363893	46.585613
2961.026023	160839.194098	46.590618
2957.382626	159956.700732	46.595623
2953.329730	159077.147359	46.600628
2949.312697	158218.283120	46.605633
2944.990977	157361.629411	46.610637
2941.353774	156500.465189	46.615642
2937.455831	155665.851497	46.620647
2933.476818	154830.842407	46.625652
2929.716189	154002.098353	46.630657
2925.750009	153181.785018	46.635661
2921.728265	152364.890183	46.640666
2917.858719	151562.198568	46.645671
2913.583366	150763.068685	46.650676
2910.096009	149969.745318	46.655681
2906.091854	149201.010470	46.660685
2902.265449	148421.442616	46.665690
2898.047548	147656.021097	46.670695
2893.693273	146902.567930	46.675700
2889.682256	146165.665291	46.680705
2885.612973	145431.518084	46.685709
2881.413459	144704.883651	46.690714
2877.989184	143992.784537	46.695719
2873.943487	143285.042091	46.700724
2869.851787	142593.806931	46.705729
2865.772942	141904.004561	46.710733
2861.344660	141222.663806	46.715738
2857.427983	140548.963339	46.720743
2853.387679	139903.511322	46.725748
2849.496136	139255.538525	46.730753
2845.222942	138622.226976	46.735757
2841.533748	137996.034079	46.740762
2837.912616	137374.749868	46.745767
2833.978618	136762.759031	46.750772
2830.290137	136152.977245	46.755777
2826.308895	135574.048817	46.760781
2822.618965	134898.766590	46.765786
2818.345195	134290.424096	46.770791
2814.639144	133722.480843	46.775796
2810.875542	133136.744195	46.780801
2806.817256	132570.982296	46.785805
2803.368008	132015.067921	46.790810
2799.695781	131453.967160	46.795815
2796.066041	130903.679515	46.800820
2792.482436	130352.552200	46.805825
2788.895977	129812.486289	46.810829
2784.998821	129263.609743	46.815834
2782.041694	128721.475496	46.820839
2778.005202	128196.815012	46.825844
2774.537116	127655.282880	46.830849
2770.909194	127130.139801	46.835853
2767.500536	126589.986050	46.840858
2763.841460	126057.001040	46.845863
2760.220594	125535.540346	46.850868
2756.904053	125007.132726	46.855873
2752.795007	124482.594598	46.860877
2749.375976	123962.966982	46.865882
2745.840236	123447.395957	46.870887
2742.373585	122929.378995	46.875892
2738.968756	122412.147701	46.880897
2735.070316	121892.214836	46.885901
2731.661905	121375.455588	46.890906
2728.132916	120866.161625	46.895911
2724.506653	120349.895015	46.900916
2721.535945	119835.097489	46.905921
2717.755870	119327.719585	46.910925
2714.198119	118809.542766	46.915930
2710.811151	118292.363749	46.920935
2707.039823	117774.870121	46.925940
2703.819326	117268.297382	46.930945
2699.718244	116757.913841	46.935949
2696.417217	116250.133967	46.940954
2692.742622	115734.408299	46.945959
2689.043190	115238.949466	46.950964
2685.611513	114734.745642	46.955969
2681.809847	114231.127655	46.960973
2678.448350	113718.039048	46.965978
2675.395119	113228.101496	46.970983
2671.354635	112728.076238	46.975988
2667.821975	112236.179719	46.980993
2664.258158	111734.606532	46.985997
2660.445185	111229.252233	46.991002
2657.087930	110736.242981	46.996007
2653.314089	110250.221703	47.001012
2649.797535	109764.141671	47.006017
2646.194091	109272.119326	47.011021
2642.146443	108787.648408	47.016026
2638.754902	108306.514658	47.021031
2634.967022	107819.753918	47.026036
2631.327259	107354.880936	47.031041
2627.232100	106884.389919	47.036045
2623.293368	106434.818242	47.041050
2619.881282	105965.034478	47.046055
2615.790797	105510.871415	47.051060
2612.369039	105066.779843	47.056065
2608.733114	104612.456445	47.061069
2604.972812	104169.878539	47.066074
2601.406662	103717.005543	47.071079
2597.382859	103290.954169	47.076084
2594.119657	102855.269378	47.081089
2590.090267	102425.925151	47.086093
2586.267024	102013.535873	47.091098
2582.629773	101584.561062	47.096103
2578.996888	101169.572554	47.101108
2575.194193	100750.395981	47.106113
2571.480678	100344.950451	47.111117
2568.390953	99940.124674	47.116122
2564.818214	99537.387271	47.121127
2560.653313	99134.492874	47.126132
2557.137534	98731.019567	47.131137
2554.023851	98326.802480	47.136141
2550.231221	97924.945681	47.141146
2547.081295	97528.306263	47.146151
2543.703888	97134.287085	47.151156
2540.141143	96725.496187	47.156161
2536.714830	96320.984807	47.161165
2533.029518	95923.991396	47.166170
2529.575189	95513.242356	47.171175
2526.372847	95118.776471	47.176180
2522.713153	94715.224479	47.181185
2519.630674	94318.310229	47.186189
2516.131313	93913.879625	47.191194
2512.790824	93509.620219	47.196199
2508.948813	93102.203880	47.201204
2505.495757	92686.295047	47.206209
2502.032768	92291.245194	47.211213
2498.706323	91884.565411	47.216218
2495.264310	91469.510135	47.221223
2491.692286	91063.692809	47.226228
2488.346925	90660.475829	47.231233
2484.646604	90250.191498	47.236237
2481.042310	89838.119046	47.241242
2477.490458	89422.867736	47.246247
2474.518003	89015.701598	47.251252
2471.019260	88604.722457	47.256257
2467.268024	88200.572795	47.261261
2463.645570	87787.273853	47.266266
2460.808390	87366.934475	47.271271
2457.078758	86962.506262	47.276276
2453.809831	86531.752168	47.281281
2450.147090	86123.145467	47.286285
2446.496460	85700.873200	47.291290
2442.992755	85288.683702	47.296295
2439.425549	84875.163391	47.301300
2435.953997	84451.001405	47.306305
2432.544404	84033.238453	47.311309
2428.630458	83624.452195	47.316314
2425.468765	83198.914024	47.321319
2422.380056	82795.016151	47.326324
2418.945976	82364.223168	47.331329
2415.386459	81946.196631	47.336333
2411.836636	81518.025829	47.341338
2408.347493	81097.066770	47.346343
2405.011625	80665.179433	47.351348
2401.355173	80242.811268	47.356353
2398.078143	79827.566692	47.361357
2394.470040	79397.278228	47.366362
2391.109888	78972.355746	47.371367
2387.287104	78540.856625	47.376372
2383.688206	78109.050012	47.381377
2380.115168	77695.077409	47.386381
2376.418614	77257.546162	47.391386
2373.240029	76835.854313	47.396391
2369.398460	76420.075949	47.401396
2366.209154	75994.030123	47.406401
2363.013347	75565.477547	47.411405
2359.373898	75148.010960	47.416410
2356.349354	74696.879198	47.421415
2352.386126	74279.997143	47.426420
2349.027756	73839.979647	47.431425
2345.544198	73398.427000	47.436429
2341.813661	72973.808583	47.441434
2338.382031	72544.045895	47.446439
2334.811843	72122.158923	47.451444
2331.278005	71684.959881	47.456449
2327.932642	71252.639920	47.461453
2324.046138	70820.106572	47.466458
2321.001019	70390.439547	47.471463
2317.359802	69965.094002	47.476468
2313.984404	69525.240113	47.481473
2310.499956	69090.654192	47.486477
2307.003290	68655.912429	47.491482
2303.656620	68219.688288	47.496487
2300.013393	67786.882028	47.501492
2296.569909	67345.907915	47.506497
2293.290701	66906.096489	47.511501
2289.591999	66469.284113	47.516506
2285.951608	66032.209925	47.521511
2282.455125	65600.173282	47.526516
2279.338378	65155.523947	47.531521
2275.585750	64728.670561	47.536525
2271.938250	64282.500750	47.541530
2268.864337	63838.388482	47.546535
2264.845865	63400.752400	47.551540
2261.654161	62953.538934	47.556545
2258.160630	62516.058835	47.561549
2254.324801	62076.501005	47.566554
2251.491035	61636.547534	47.571559
2248.020320	61193.267782	47.576564
2244.388993	60744.861710	47.581569
2240.905957	60305.674029	47.586573
2237.028445	59864.334602	47.591578
2233.432850	59414.253036	47.596583
2229.845077	58974.674111	47.601588
2226.306600	58529.416316	47.606593
2223.417501	58080.461513	47.611597
2219.324666	57626.562786	47.616602
2216.264461	57190.138538	47.621607
2212.460664	56758.000242	47.626612
2208.744084	56306.333079	47.631617
2205.503103	55856.408690	47.636621
2202.103708	55423.026122	47.641626
2198.733412	54964.078636	47.646631
2195.282866	54527.478358	47.651636
2191.889392	54070.486846	47.656641
2188.441477	53626.708451	47.661645
2184.567487	53178.297493	47.666650
2181.356945	52729.011565	47.671655
2177.690266	52282.355452	47.676660
2174.124306	51830.306470	47.681665
2170.739509	51375.795828	47.686669
2167.451396	50926.969068	47.691674
2163.861894	50476.884864	47.696679
2159.953953	50035.409564	47.701684
2156.913449	49584.058504	47.706689
2153.040823	49121.644262	47.711693
2149.967702	48674.217073	47.716698
2146.087009	48215.653449	47.721703
2142.409708	47776.443807	47.726708
2138.921639	47316.416486	47.731713
2135.801758	46871.974896	47.736717
2132.220561	46416.889274	47.741722
2128.844599	45972.219858	47.746727
2125.246467	45520.503579	47.751732
2121.402758	45066.114003	47.756737
2118.315308	44620.659132	47.761741
2114.638758	44161.099859	47.766746
2111.882857	43704.856503	47.771751
2108.167537	43251.600030	47.776756
2104.463555	42777.545882	47.781761
2100.960041	42324.262773	47.786765
2097.612661	41869.480935	47.791770
2093.699373	41416.743182	47.796775
2090.440577	40955.746249	47.801780
2086.825004	40493.597196	47.806785
2083.270562	40037.123007	47.811789
2079.846151	39577.182761	47.816794
2076.029698	39117.788783	47.821799
2072.436177	38661.907535	47.826804
2068.838793	38199.595299	47.831809
2065.792671	37759.865094	47.836813
2062.301495	37299.812584	47.841818
2058.903383	36843.489361	47.846823
2055.024655	36379.117430	47.851828
2051.843190	35929.410875	47.856833
2048.220609	35467.174262	47.861837
2044.864068	35010.085141	47.866842
2041.430334	34545.081857	47.871847
2037.646323	34099.894276	47.876852
2034.073445	33624.556723	47.881857
2030.582619	33168.891168	47.886861
2027.029700	32714.107171	47.891866
2023.401682	32251.580699	47.896871
2019.951556	31795.032416	47.901876
2016.867989	31335.654840	47.906881
2012.903359	30881.127039	47.911885
2009.223223	30428.111278	47.916890
2005.513083	29966.827262	47.921895
2001.834052	29523.153378	47.926900
1999.094287	29065.300029	47.931905
1995.757212	28616.953797	47.936909
1991.907926	28161.694997	47.941914
1988.641397	27703.282400	47.946919
1984.551175	27251.718629	47.951924
1981.171682	26786.108036	47.956929
1977.608845	26334.425571	47.961933
1973.753344	25883.248602	47.966938
1970.607549	25426.471711	47.971943
1967.387715	24986.259357	47.976948
1963.880160	24526.283628	47.981953
1960.148603	24080.627129	47.986957
1956.161369	23626.512013	47.991962
1953.022075	23176.380467	47.996967
1949.100830	22736.485190	48.001972
1945.867836	22281.345798	48.006977
1941.990758	21836.965824	48.011981
1938.479629	21404.574657	48.016986
1935.214156	20956.755625	48.021991
1931.447633	20510.747701	48.026996
1927.843124	20072.015343	48.032001
1924.287984	19622.124539	48.037005
1920.394310	19195.814551	48.042010
1917.167352	18758.604715	48.047015
1913.636836	18316.575055	48.052020
1909.834634	17885.225313	48.057025
1906.068209	17448.698935	48.062029
1902.199553	17021.580951	48.067034
1898.998857	16603.893383	48.072039
1895.013187	16193.391918	48.077044
1891.284975	15768.024604	48.082049
1887.523376	15363.272021	48.087053
1883.647430	14956.687203	48.092058
1879.436359	14564.426894	48.097063
1875.111902	14182.304922	48.102068
1870.976535	13796.532890	48.107073
1867.286014	13432.614534	48.112077
1863.549676	13073.490874	48.117082
1859.987542	12713.156545	48.122087
1855.846895	12359.801633	48.127092
1852.172009	12009.334516	48.132097
1848.461161	11666.891930	48.137101
1844.681982	11326.251648	48.142106
1841.307948	10985.469026	48.147111
1837.702803	10656.171992	48.152116
1834.317682	10322.234406	48.157121
1830.816426	9993.967987	48.162125
1826.727250	9678.245095	48.167130
1823.631679	9350.110477	48.172135
1819.474004	9035.839881	48.177140
1816.143532	8706.167406	48.182145
1812.713140	8399.508020	48.187149
1809.317851	8084.628485	48.192154
1805.675564	7762.465679	48.197159
1802.044759	7454.678942	48.202164
1798.600031	7132.205229	48.207169
1795.016667	6822.380303	48.212173
1791.378072	6515.436540	48.217178
1787.843060	6193.961797	48.222183
1784.246214	5903.282423	48.227188
1780.825114	5592.155515	48.232193
1777.259610	5297.015562	48.237197
1774.203156	5012.073358	48.242202
1770.313291	4698.927051	48.247207
1766.461798	4416.459662	48.252212
1762.949510	4110.574659	48.257217
1759.018712	3828.711024	48.262221
1754.870021	3547.259084	48.267226
1751.367816	3264.878708	48.272231
1747.288388	3016.924385	48.277236
1742.892391	2765.665552	48.282241
1739.165086	2517.881630	48.287245
1734.814473	2276.548470	48.292250
1731.117860	2048.554500	48.297255
1726.989193	1832.024291	48.302260
1723.466353	1618.730915	48.307265
1719.741940	1407.844411	48.312269
1715.424930	1210.863073	48.317274
1711.971394	1008.124157	48.322279
1707.713778	818.522385	48.327284
1703.966404	631.235054	48.332289
1700.215420	465.147528	48.337293
1696.039425	298.729073	48.342298
1692.106893	151.000324	48.347303
1686.827616	33.132559	48.352308
1677.035984	58.577481	48.357313
1669.528356	67.130268	48.362317
1665.001336	69.249243	48.367322
1662.363265	70.314928	48.372327
1659.605756	67.798910	48.377332
1657.520311	72.597172	48.382337
1654.780248	71.198389	48.387341
1651.956897	69.584784	48.392346
1649.556937	67.677494	48.397351
1646.288339	67.936498	48.402356
1642.394045	72.595524	48.407361
1638.985451	74.695447	48.412365
1635.130188	77.209736	48.417370
1631.946292	74.070396	48.422375
1628.585722	71.236962	48.427380
1625.298909	78.762664	48.432385
1622.441881	76.148244	48.437389
1618.411339	85.789167	48.442394
1615.412123	73.835480	48.447399
1612.050550	73.976083	48.452404
1608.545610	82.190624	48.457409
1605.039841	81.809513	48.462413
1601.534233	84.250402	48.467418
1598.443682	67.457818	48.472423
1594.932863	73.629520	48.477428
1591.058186	70.366752	48.482433
1588.132390	75.289484	48.487437
1584.540319	73.181773	48.492442
1581.010980	71.921662	48.497447
1577.677815	77.724035	48.502452
1574.130430	79.083114	48.507457
1570.534146	73.787049	48.512461
1566.863114	76.813661	48.517466
1563.837573	70.609366	48.522471
1560.307602	77.369337	48.527476
1557.198790	78.024251	48.532481
1553.891501	72.161197	48.537485
1549.869609	75.805560	48.542490
1546.514142	72.341764	48.547495
1542.654462	71.142564	48.552500
1539.610812	69.892281	48.557505
1535.996203	70.477229	48.562509
1532.518843	81.405096	48.567514
1529.482712	77.081690	48.572519
1525.634022	85.210535	48.577524
1521.672716	78.082560	48.582529
1518.662352	79.136599	48.587533
1515.096857	87.202385	48.592538
1512.121140	71.426474	48.597543
1508.331826	82.839487	48.602548
1504.948863	79.560305	48.607553
1501.855052	70.022614	48.612557
1498.099023	79.604991	48.617562
1494.407139	71.615691	48.622567
1490.921438	73.411258	48.627572
1486.875401	75.097890	48.632577
1483.764468	77.885473	48.637581
1480.154422	78.210293	48.642586
1477.201142	71.697374	48.647591
1473.584791	78.815636	48.652596
1470.063486	80.825551	48.657601
1466.733732	78.199305	48.662605
1462.854861	81.653738	48.667610
1459.521888	78.787553	48.672615
1456.040719	83.062758	48.677620
1452.229304	75.522331	48.682625
1449.218450	81.312508	48.687629
1445.638907	81.436434	48.692634
1442.278323	73.028587	48.697639
1438.828374	78.494809	48.702644
1435.172127	77.792295	48.707649
1431.911739	75.316606	48.712653
1427.733680	77.795735	48.717658
1424.919085	71.780085	48.722663
1421.171558	74.068819	48.727668
1417.402556	81.444957	48.732673
1414.136377	78.593691	48.737677
1410.267867	74.102472	48.742682
1407.294053	69.212574	48.747687
1403.661862	79.376779	48.752692
1400.340383	76.167134	48.757697
1397.048035	70.067665	48.762701
1393.464665	79.230871	48.767706
1389.660740	67.668235	48.772711
1385.976048	79.840068	48.777716
1382.584182	78.960370	48.782721
1379.522314	75.273729	48.787725
1375.522164	72.024192	48.792730
1372.374561	72.947747	48.797735
1368.415567	90.407690	48.802740
1365.239974	81.480684	48.807745
1361.989248	75.282993	48.812749
1358.646173	81.216631	48.817754
1355.557899	73.212494	48.822759
1351.757240	72.064241	48.827764
1347.678402	79.216531	48.832769
1343.559653	79.592071	48.837773
1340.120427	75.559217	48.842778
1337.313883	68.795694	48.847783
1333.676255	76.338044	48.852788
1330.467384	73.756274	48.857793
1326.972098	77.834371	48.862797
1323.587808	75.839879	48.867802
1319.837363	75.579139	48.872807
1316.071612	71.973594	48.877812
1313.049729	71.441268	48.882817
1309.568027	68.797565	48.887821
1305.875583	70.435506	48.892826
1302.735927	64.941861	48.897831
1298.741717	73.093360	48.902836
1295.237787	71.807180	48.907841
1291.991085	63.669534	48.912845
1288.236302	77.990931	48.917850
1285.024634	66.462680	48.922855
1281.153954	75.933195	48.927860
1277.463315	73.261908	48.932865
1274.315206	64.403414	48.937869
1270.760487	67.585947	48.942874
1267.463683	67.662719	48.947879
1263.773721	71.033980	48.952884
1259.912378	79.031928	48.957889
1256.929289	70.312260	48.962893
1253.300841	78.745347	48.967898
1250.091721	62.360440	48.972903
1246.572167	71.988268	48.977908
1243.024496	72.395150	48.982913
1239.413077	69.268621	48.987917
1235.618066	70.631473	48.992922
1232.412331	66.584439	48.997927
1228.866099	69.781474	49.002932
1225.247335	72.357061	49.007937
1222.144200	68.344677	49.012941
1218.208387	62.500417	49.017946
1214.665614	65.314107	49.022951
1211.011834	68.973964	49.027956
1207.780673	66.515899	49.032961
1204.129180	64.556688	49.037965
1201.060597	71.450494	49.042970
1197.555206	67.383670	49.047975
1193.896601	73.113333	49.052980
1190.200979	79.683974	49.057985
1186.819666	65.489847	49.062989
1183.427031	71.032581	49.067994
1179.901476	60.027766	49.072999
1176.473229	68.018409	49.078004
1172.691561	71.350170	49.083009
1169.363363	73.991263	49.088013
1165.787403	71.994989	49.093018
1162.734662	57.847804	49.098023
1159.178025	62.720054	49.103028
1155.271744	70.111242	49.108033
1151.758171	63.720388	49.113037
1148.117922	74.920377	49.118042
1145.142146	61.754612	49.123047
1141.551274	66.717612	49.128052
1137.498136	62.343761	49.133057
1134.286513	62.385142	49.138061
1130.590811	66.538738	49.143066
1127.474505	73.218518	49.148071
1124.019858	70.238441	49.153076
1120.526536	70.994373	49.158081
1117.132227	63.556762	49.163085
1113.467956	69.284148	49.168090
1109.807115	73.027368	49.173095
1105.889988	63.051607	49.178100
1102.586046	61.620429	49.183105
1099.226062	65.892609	49.188109
1095.750499	70.787045	49.193114
1092.519916	69.116663	49.198119
1088.772537	63.470879	49.203124
1085.275368	70.981884	49.208129
1081.722794	66.992023	49.213133
1078.180795	71.292538	49.218138
1074.674745	59.857612	49.223143
1071.352845	61.308186	49.228148
1068.141940	62.440932	49.233153
1064.758909	60.930323	49.238157
1060.945950	67.645780	49.243162
1057.687550	61.942870	49.248167
1053.947887	65.432614	49.253172
1050.063705	64.142380	49.258177
1046.648428	62.646283	49.263181
1043.137186	62.690020	49.268186
1039.759724	59.068370	49.273191
1036.231239	63.237072	49.278196
1032.416501	69.411818	49.283201
1029.029863	62.090086	49.288205
1025.548628	69.101914	49.293210
1022.660367	75.863258	49.298215
1019.266586	69.362030	49.303220
1015.231787	71.562645	49.308225
1011.799268	70.391932	49.313229
1008.110809	70.131071	49.318234
1005.111424	60.474374	49.323239
1001.332364	63.691851	49.328244
997.754663	67.232318	49.333249
994.422701	64.619133	49.338253
990.376367	66.751944	49.343258
987.204166	59.839756	49.348263
983.535468	55.858498	49.353268
980.262040	59.446511	49.358273
976.993012	61.233705	49.363277
973.246146	70.915906	49.368282
969.801664	73.125874	49.373287
966.583547	69.507901	49.378292
962.758479	69.679590	49.383297
959.492822	63.999970	49.388301
955.444799	63.159188	49.393306
952.250403	62.963793	49.398311
948.761984	61.574005	49.403316
945.072787	69.405966	49.408321
941.814814	68.318820	49.413325
938.101554	73.266087	49.418330
934.444902	59.905806	49.423335
931.010785	60.807563	49.428340
927.394639	74.382892	49.433345
924.588617	66.363368	49.438349
920.907671	69.777548	49.443354
917.539579	70.036293	49.448359
913.595592	67.407659	49.453364
910.019992	75.032121	49.458369
906.485448	63.557373	49.463373
902.769822	70.665805	49.468378
899.793459	62.040067	49.473383
896.735496	66.822056	49.478388
892.914432	63.794650	49.483393
889.416624	58.265074	49.488397
885.472863	58.442595	49.493402
882.188660	57.486087	49.498407
879.017575	57.786933	49.503412
875.178407	61.928082	49.508417
871.548657	65.530445	49.513421
867.891981	70.579638	49.518426
864.569650	62.482314	49.523431
861.117483	60.102989	49.528436
857.690831	62.791071	49.533441
854.257974	66.381768	49.538445
850.300372	64.622112	49.543450
847.269495	54.201576	49.548455
843.759374	54.653277	49.553460
840.068702	63.690833	49.558465
836.568494	55.763572	49.563469
833.238783	64.327334	49.568474
829.684789	57.436642	49.573479
826.159888	60.510170	49.578484
822.621605	55.597497	49.583489
819.330918	64.933449	49.588493
815.466729	62.852382	49.593498
812.303087	59.418937	49.598503
808.773503	68.165672	49.603508
804.966277	67.078624	49.608513
801.591219	58.043581	49.613517
797.777659	59.997814	49.618522
794.820746	60.796828	49.623527
791.060140	60.411189	49.628532
787.580872	66.559040	49.633537
784.350782	54.426341	49.638541
780.347918	55.995603	49.643546
776.968228	60.068399	49.648551
773.739977	64.402353	49.653556
769.838527	74.042191	49.658561
766.855576	64.044465	49.663565
763.059025	60.851917	49.668570
759.796196	61.622627	49.673575
755.903551	60.223025	49.678580
752.006278	60.485074	49.683585
748.845621	63.422817	49.688589
745.534043	59.727680	49.693594
741.803239	56.252826	49.698599
738.943264	59.785988	49.703604
735.700400	61.866518	49.708609
731.963417	60.790692	49.713613
728.095979	68.160044	49.718618
724.397961	60.010501	49.723623
720.603265	65.482978	49.728628
717.826885	65.089663	49.733633
713.968898	58.837922	49.738637
710.348795	64.058599	49.743642
707.106382	62.298361	49.748647
703.867773	65.080568	49.753652
700.092665	60.128853	49.758657
696.964790	57.234009	49.763661
693.105659	66.987480	49.768666
689.688820	54.953474	49.773671
686.117910	63.345987	49.778676
682.287579	64.967496	49.783681
679.101795	56.266837	49.788685
675.303397	70.009739	49.793690
672.062169	59.277140	49.798695
668.613335	58.612035	49.803700
664.356091	59.078827	49.808705
661.651847	52.353270	49.813709
658.010591	52.743152	49.818714
654.313181	59.108463	49.823719
650.885365	63.264690	49.828724
647.527295	59.893173	49.833729
644.366922	53.751141	49.838733
640.405950	64.694190	49.843738
636.739283	59.048578	49.848743
633.891627	55.584951	49.853748
629.773602	65.562221	49.858753
626.279061	58.640165	49.863757
622.496240	67.976811	49.868762
619.771469	73.339685	49.873767
615.955734	65.316053	49.878772
612.083808	74.343879	49.883777
609.138478	69.535078	49.888781
605.426393	67.287999	49.893786
601.845999	66.928114	49.898791
598.269152	65.409773	49.903796
594.768241	66.749062	49.908801
591.664860	58.181120	49.913805
587.888691	63.704507	49.918810
584.177332	61.017568	49.923815
581.017623	62.449271	49.928820
577.635188	63.950448	49.933825
574.200434	65.712863	49.938829
570.285836	66.044072	49.943834
566.958029	64.214891	49.948839
563.510829	66.947329	49.953844
560.076328	68.266793	49.958849
556.524009	61.553056	49.963853
552.803986	68.772925	49.968858
549.259717	61.055052	49.973863
545.934199	62.234168	49.978868
542.143826	70.825370	49.983873
538.739213	63.626744	49.988877
534.834665	67.401631	49.993882
531.947022	67.313550	49.998887
528.610222	62.407523	50.003892
525.071491	58.453562	50.008897
521.874999	59.036806	50.013901
517.725803	67.446594	50.018906
513.987704	59.189443	50.023911
510.884437	58.090922	50.028916
507.170368	56.625595	50.033921
504.086562	49.272639	50.038925
500.251650	61.936085	50.043930
496.907452	54.629993	50.048935
493.680810	55.822195	50.053940
489.672765	69.154824	50.058945
486.414878	55.707269	50.063949
483.028131	64.558329	50.068954
479.212981	55.060370	50.073959
475.741367	54.674078	50.078964
472.289765	56.717530	50.083969
468.799804	57.596398	50.088973
465.385762	62.335777	50.093978
461.936387	54.486096	50.098983
458.248320	57.009276	50.103988
454.863304	50.044897	50.108993
451.247548	54.749241	50.113997
447.617915	61.556422	50.119002
444.156879	51.870470	50.124007
440.707028	49.585759	50.129012
437.390668	52.655334	50.134017
433.886577	57.680809	50.139021
430.032174	57.056731	50.144026
426.924172	55.829248	50.149031
423.487674	55.371058	50.154036
419.591665	54.582621	50.159041
416.441103	53.735079	50.164045
412.771902	65.129412	50.169050
409.096360	60.127449	50.174055
405.877261	57.490452	50.179060
402.026595	64.667397	50.184065
398.820533	52.727193	50.189069
395.193620	50.875003	50.194074
391.668385	55.229912	50.199079
388.492278	44.721357	50.204084
384.659647	59.469305	50.209089
381.174424	55.488057	50.214093
377.594158	51.632335	50.219098
374.263862	61.294001	50.224103
370.832364	55.472628	50.229108
366.855894	60.052810	50.234113
363.841679	52.584643	50.239117
359.889483	60.229801	50.244122
356.675973	58.338565	50.249127
353.020360	53.596097	50.254132
349.606004	56.756866	50.259137
346.292811	51.844034	50.264141
343.144779	50.869561	50.269146
339.412843	57.547148	50.274151
336.215483	57.526290	50.279156
332.113949	58.750318	50.284161
328.677650	47.905806	50.289165
324.623317	60.043450	50.294170
321.927302	50.266897	50.299175
317.942086	53.497561	50.304180
314.382493	55.269952	50.309185
311.203693	47.719855	50.314189
307.586771	52.747089	50.319194
303.944300	62.416231	50.324199
300.764819	52.917424	50.329204
296.801032	65.249779	50.334209
293.652920	56.581294	50.339213
290.135015	57.872648	50.344218
286.490905	55.153145	50.349223
283.399543	55.685251	50.354228
279.367357	54.816801	50.359233
276.348102	54.546766	50.364237
272.460261	70.967407	50.369242
269.009345	58.612946	50.374247
265.741481	59.583809	50.379252
262.226833	61.592811	50.384257
258.853094	54.092054	50.389261
254.950847	63.314440	50.394266
251.323837	62.911245	50.399271
248.112885	62.266109	50.404276
244.586173	57.057516	50.409281
241.336519	55.693928	50.414285
237.763622	67.335861	50.419290
234.112601	63.655688	50.424295
230.545900	56.086905	50.429300
226.796251	52.270235	50.434305
223.380000	46.032081	50.439309
219.966800	57.421362	50.444314
216.404719	63.022182	50.449319
213.200537	55.994894	50.454324
209.738832	57.236381	50.459329
206.195227	59.091715	50.464333
202.267116	63.566316	50.469338
198.813289	62.959000	50.474343
195.375689	57.701741	50.479348
191.958817	59.388654	50.484353
188.838670	57.618945	50.489357
185.487012	57.422819	50.494362
181.393387	56.889808	50.499367
178.100599	57.437468	50.504372
174.543914	59.570081	50.509377
171.233850	54.134789	50.514381
167.450887	61.089249	50.519386
163.996494	58.988779	50.524391
160.737814	54.342731	50.529396
157.012144	55.033718	50.534401
153.389071	49.979348	50.539405
149.905236	59.851585	50.544410
146.393206	50.724117	50.549415
143.109265	53.643147	50.554420
139.221784	60.923921	50.559425
136.023388	51.953262	50.564429
132.543623	56.452975	50.569434
129.005845	49.041059	50.574439
125.736238	48.335473	50.579444
121.926914	57.015070	50.584449
118.518311	49.684282	50.589453
114.645719	47.693224	50.594458
111.455333	52.040319	50.599463
107.849553	49.922303	50.604468
104.234640	57.625699	50.609473
101.387395	52.504328	50.614477
97.743136	67.665874	50.619482
93.967504	61.749440	50.624487
90.656570	61.021820	50.629492
86.849915	65.743272	50.634497
83.254568	59.115421	50.639501
79.599648	62.826189	50.644506
76.196547	60.565892	50.649511
73.100731	59.320742	50.654516
69.421424	61.364896	50.659521
66.291951	60.533099	50.664525
62.238891	56.596026	50.669530
58.899282	57.264883	50.674535
55.850944	59.827713	50.679540
51.962815	62.685806	50.684545
48.285077	54.890749	50.689549
44.760610	61.463299	50.694554
41.171315	50.304163	50.699559
37.856954	49.662504	50.704564
34.179064	60.934824	50.709569
30.954641	50.247211	50.714573
27.413676	56.787531	50.719578
24.074904	55.058212	50.724583
20.479078	57.301340	50.729588
16.875045	60.871318	50.734593
13.641589	46.964518	50.739597
9.861788	59.749114	50.744602
6.218794	48.171256	50.749607
3.078115	47.575323	50.754612