Fri Aug 26 11:46:48 2022

Number of Points = 9929

Depth (nm)	Load (N)	Time (s)
0.354250	99.601738	0.000000
0.526304	99.445293	0.005005
0.110712	82.701533	0.010010
-0.102151	81.064318	0.015014
-0.309166	78.435968	0.020019
-0.320932	59.190177	0.025024
-0.935623	68.697808	0.030029
-0.883221	63.301999	0.035034
-1.090331	57.225284	0.040038
-1.520779	53.072045	0.045043
-1.168033	42.706838	0.050048
-2.341356	40.146690	0.055053
-1.952975	34.097486	0.060058
-2.504227	34.939481	0.065062
-2.965572	23.850015	0.070067
-2.795261	13.896030	0.075072
-3.154502	11.446410	0.080077
-3.479246	3.385442	0.085082
-3.652972	6.563534	0.090086
-3.479901	4.151254	0.095091
-4.235234	0.962904	0.100096
-4.733768	-6.403472	0.105101
-4.839044	-12.502345	0.110106
-5.376439	-11.520146	0.115110
-5.761399	-14.557359	0.120115
-5.642951	-12.221999	0.125120
-5.788283	-9.083131	0.130125
-6.979190	-13.674753	0.135130
-7.376862	-5.627753	0.140134
-7.601079	-10.021886	0.145139
-7.105793	-16.631865	0.150144
-7.262817	-9.805536	0.155149
-7.473454	-16.093640	0.160154
-7.455753	-7.978440	0.165158
-7.700665	-12.951461	0.170163
-8.377982	-9.403910	0.175168
-8.889945	-7.236141	0.180173
-8.808296	-15.028192	0.185178
-8.767365	-13.332473	0.190182
-9.336399	-10.934364	0.195187
-10.022174	-12.940848	0.200192
-10.553723	-14.844799	0.205197
-10.563131	-9.041164	0.210202
-10.374465	-10.323287	0.215206
-10.804407	-7.095815	0.220211
-10.260609	-12.463709	0.225216
-10.900758	-5.720339	0.230221
-11.663261	-10.141390	0.235226
-11.931030	-9.432117	0.240230
-12.080349	-9.443615	0.245235
-12.107849	-10.065680	0.250240
-11.954201	-5.122632	0.255245
-12.510962	-7.123895	0.260250
-13.473026	-8.745689	0.265254
-13.554252	-2.124141	0.270259
-13.477266	-4.878952	0.275264
-13.581208	3.922721	0.280269
-13.527577	-11.859493	0.285274
-13.814674	-4.177710	0.290278
-14.333205	-3.188956	0.295283
-14.462641	-11.916217	0.300288
-15.018185	-11.196938	0.305293
-15.131858	-7.983909	0.310298
-15.033211	-9.739216	0.315302
-15.701815	-5.364147	0.320307
-15.969122	-10.918954	0.325312
-16.345691	-6.927864	0.330317
-16.200549	-12.385543	0.335322
-16.562233	-14.183069	0.340326
-17.323070	-12.039824	0.345331
-17.399124	-13.188985	0.350336
-17.946492	-3.540021	0.355341
-17.765157	-8.373771	0.360346
-18.022617	-13.490365	0.365350
-18.203934	-10.519895	0.370355
-18.061660	-7.248643	0.375360
-18.551885	-9.320374	0.380365
-19.420986	-5.818889	0.385370
-19.814757	-5.093161	0.390374
-19.233121	-3.326609	0.395379
-19.173733	-6.860099	0.400384
-19.584862	-9.102327	0.405389
-20.133712	-9.323691	0.410394
-20.601274	-12.604298	0.415398
-21.019772	-11.235664	0.420403
-20.758144	-14.152094	0.425408
-21.000476	-12.260417	0.430413
-20.903866	-5.878524	0.435418
-21.775085	-14.177088	0.440422
-22.680311	-10.980016	0.445427
-22.232263	-11.404050	0.450432
-22.821016	-9.739999	0.455437
-22.316225	-13.814218	0.460442
-22.527069	-12.373516	0.465446
-23.430011	-10.739637	0.470451
-23.566099	-11.287850	0.475456
-23.803185	-8.533315	0.480461
-23.839733	-19.533873	0.485466
-24.005581	-11.304680	0.490470
-24.224252	-14.763238	0.495475
-24.512229	-17.919949	0.500480
-25.142560	2.039583	0.505485
-25.211838	-9.658214	0.510490
-25.157329	-21.207604	0.515494
-25.634836	-0.933360	0.520499
-25.881793	-11.831562	0.525504
-26.609485	-5.036599	0.530509
-26.795692	-9.613814	0.535514
-26.788436	-11.443474	0.540518
-26.765892	-14.303697	0.545523
-26.815071	-19.522318	0.550528
-27.232108	-7.346919	0.555533
-27.709635	-9.933137	0.560538
-27.651485	-14.633814	0.565542
-27.968023	-4.337445	0.570547
-28.091953	-9.712103	0.575552
-29.017768	-4.885713	0.580557
-29.686838	-5.477487	0.585562
-29.556580	-12.660195	0.590566
-29.669446	-12.756460	0.595571
-29.383000	-18.014683	0.600576
-30.029561	-6.243293	0.605581
-29.720015	-15.738064	0.610586
-30.356491	-11.073780	0.615590
-30.900481	-12.602484	0.620595
-30.839705	-17.420624	0.625600
-31.312363	-8.957006	0.630605
-31.492949	-12.026038	0.635610
-31.587823	-8.496409	0.640614
-32.436237	1.281685	0.645619
-32.517707	-0.265252	0.650624
-32.634516	-1.892105	0.655629
-32.658568	-7.263333	0.660634
-32.689984	-0.260413	0.665638
-32.996188	3.621651	0.670643
-33.361150	-5.148032	0.675648
-34.337077	-7.950867	0.680653
-34.315403	0.989426	0.685658
-34.443710	-7.291938	0.690662
-34.327705	-5.244089	0.695667
-33.913287	-4.299358	0.700672
-35.117797	-4.133908	0.705677
-35.485548	2.529088	0.710682
-35.533518	-4.888456	0.715686
-35.520402	-2.596805	0.720691
-35.772903	-7.198498	0.725696
-35.689627	-2.639949	0.730701
-36.342552	-1.753652	0.735706
-36.438685	-2.017031	0.740710
-36.863427	-5.326451	0.745715
-37.253076	-11.915701	0.750720
-37.650547	-7.570192	0.755725
-38.339455	-11.885645	0.760730
-38.439645	-5.530057	0.765734
-38.581481	-3.125697	0.770739
-38.611934	-5.541087	0.775744
-38.731078	-2.061459	0.780749
-38.779093	1.422912	0.785754
-38.783364	-3.793214	0.790758
-39.465875	3.083300	0.795763
-39.693063	-13.597951	0.800768
-40.135565	-7.812303	0.805773
-39.959095	-7.776453	0.810778
-40.152247	-9.568582	0.815782
-40.902359	-3.532565	0.820787
-41.331566	-2.709574	0.825792
-41.407315	-4.769911	0.830797
-41.504025	-8.582804	0.835802
-41.859290	-4.281830	0.840806
-41.864204	2.919437	0.845811
-41.916103	-8.626046	0.850816
-42.816033	0.334357	0.855821
-42.999518	-1.196696	0.860826
-43.019878	-3.566203	0.865830
-43.678291	1.924047	0.870835
-43.215820	-0.685146	0.875840
-43.420893	-7.100663	0.880845
-43.970634	-6.258905	0.885850
-44.285258	-8.835686	0.890854
-44.885620	-4.689533	0.895859
-44.630688	-14.080891	0.900864
-44.672588	-8.908090	0.905869
-44.840508	-16.730880	0.910874
-45.618755	-3.414112	0.915878
-46.341647	-7.996347	0.920883
-46.017126	-8.638422	0.925888
-46.091864	-3.191597	0.930893
-46.037337	-3.548033	0.935898
-46.531209	-2.892138	0.940902
-47.694792	0.247090	0.945907
-47.449799	-4.150499	0.950912
-47.814119	-8.048271	0.955917
-47.788230	-8.719776	0.960922
-47.911864	-4.812359	0.965926
-48.190194	-9.422684	0.970931
-47.998597	-10.860281	0.975936
-48.615246	-7.515157	0.980941
-49.207184	-3.705661	0.985946
-49.169614	-8.792264	0.990950
-49.471519	-7.353202	0.995955
-49.275792	-11.594427	1.000960
-50.079663	-8.862372	1.005965
-50.282776	-10.621313	1.010970
-50.441518	-10.352943	1.015974
-50.483521	-6.790418	1.020979
-50.557509	-12.258268	1.025984
-51.637077	-6.265865	1.030989
-51.740184	-9.157143	1.035994
-51.733098	-6.579826	1.040998
-51.830467	-1.787514	1.046003
-51.885598	-12.535253	1.051008
-53.020675	-5.866679	1.056013
-53.173311	-6.671734	1.061018
-53.325845	-1.152687	1.066022
-53.633553	-2.544179	1.071027
-53.409122	-11.861189	1.076032
-53.575900	-10.715240	1.081037
-53.343858	-4.746726	1.086042
-53.773987	-13.477784	1.091046
-55.020033	-2.881673	1.096051
-54.852746	-11.158439	1.101056
-54.634707	-4.909345	1.106061
-55.101640	-5.532590	1.111066
-55.746855	-4.413384	1.116070
-55.872442	2.661143	1.121075
-55.903018	-13.417990	1.126080
-56.068342	-3.293857	1.131085
-56.470466	-8.723272	1.136090
-56.985163	-5.001730	1.141094
-57.724862	-4.674541	1.146099
-57.535325	-12.287243	1.151104
-57.472617	-7.285747	1.156109
-57.776926	-11.072644	1.161114
-57.865707	-9.533893	1.166118
-58.008619	-0.881177	1.171123
-58.361526	-9.475568	1.176128
-58.813767	-6.390151	1.181133
-59.109143	-13.054187	1.186138
-58.962981	-11.839908	1.191142
-59.571002	-5.022451	1.196147
-60.019115	-16.607473	1.201152
-60.290778	-17.713521	1.206157
-60.646885	-7.268631	1.211162
-60.663239	-10.046870	1.216166
-60.888599	-3.251029	1.221171
-60.629105	-13.139789	1.226176
-60.783947	-3.099543	1.231181
-61.157166	-17.296738	1.236186
-61.854470	-18.349169	1.241190
-62.322802	-6.719423	1.246195
-61.878149	-8.354603	1.251200
-62.324860	-8.284996	1.256205
-63.411613	-6.198569	1.261210
-63.464567	-9.306456	1.266214
-63.591017	-13.446899	1.271219
-63.339641	-18.345333	1.276224
-63.730181	-12.339995	1.281229
-63.493752	-13.031627	1.286234
-64.317879	-16.332640	1.291238
-64.972690	-0.453561	1.296243
-65.188599	-9.233792	1.301248
-65.330941	-11.663396	1.306253
-65.248190	-8.329096	1.311258
-64.967602	-11.074478	1.316262
-65.291400	-2.510654	1.321267
-65.907049	-9.722752	1.326272
-66.486815	0.674712	1.331277
-66.775844	-4.639440	1.336282
-66.333536	-2.781596	1.341286
-66.996716	2.342413	1.346291
-67.702484	-9.354351	1.351296
-67.927748	-9.369841	1.356301
-68.004901	-6.782572	1.361306
-68.503513	-7.555903	1.366310
-68.728253	-5.299982	1.371315
-68.368851	-11.562948	1.376320
-68.435142	-2.121763	1.381325
-68.482816	1.444810	1.386330
-68.921807	-7.471524	1.391334
-69.676140	-6.148673	1.396339
-69.474302	-10.023868	1.401344
-70.131185	-10.408737	1.406349
-70.941861	-10.586170	1.411354
-70.948008	-15.261017	1.416358
-71.791025	-1.908856	1.421363
-70.767128	-9.281323	1.426368
-71.200847	-5.078861	1.431373
-71.468264	-6.188736	1.436378
-71.845721	-10.261625	1.441382
-72.113884	-8.808835	1.446387
-71.853729	-6.454412	1.451392
-72.305604	-0.505957	1.456397
-72.589955	-3.811925	1.461402
-72.600144	-13.994040	1.466406
-73.434910	-1.076581	1.471411
-73.647064	-12.850198	1.476416
-73.868855	-13.483139	1.481421
-73.780612	-7.868711	1.486426
-73.903439	-8.646770	1.491430
-74.974152	-6.936149	1.496435
-75.429556	-3.223839	1.501440
-75.851357	-6.676078	1.506445
-75.410543	-7.545060	1.511450
-75.620792	-3.219211	1.516454
-75.734225	-0.199201	1.521459
-75.746460	-1.152662	1.526464
-75.706781	-6.720465	1.531469
-76.826248	-5.514763	1.536474
-76.650532	-4.039339	1.541478
-77.254568	-3.258727	1.546483
-77.237261	0.705838	1.551488
-77.090570	0.727343	1.556493
-77.702745	-6.719406	1.561498
-78.264042	-5.470902	1.566502
-78.636134	-9.225098	1.571507
-78.558486	-13.460592	1.576512
-78.708541	-1.836109	1.581517
-78.831553	-4.056759	1.586522
-79.321728	-6.236060	1.591526
-80.000649	-5.820261	1.596531
-79.990505	-15.464557	1.601536
-80.400075	-0.655011	1.606541
-80.467987	0.583110	1.611546
-79.933814	-10.651838	1.616550
-80.852209	-0.147869	1.621555
-81.111295	-6.441083	1.626560
-81.423968	-3.165433	1.631565
-81.623387	-3.789203	1.636570
-81.734771	-9.140502	1.641574
-81.932287	-5.759401	1.646579
-82.388176	-16.027136	1.651584
-82.781987	-15.174856	1.656589
-82.781026	-10.733204	1.661594
-82.857138	-13.960865	1.666598
-83.174956	-0.386768	1.671603
-83.659964	-6.992806	1.676608
-84.336258	-2.489993	1.681613
-84.416836	-0.209063	1.686618
-84.733395	-4.345217	1.691622
-84.740915	-6.485776	1.696627
-84.322782	-6.342026	1.701632
-84.540580	-0.917218	1.706637
-85.211765	-1.274551	1.711642
-85.148014	-15.713781	1.716646
-85.466030	-3.022311	1.721651
-86.078219	-9.959709	1.726656
-87.174244	-6.929073	1.731661
-87.279765	0.506146	1.736666
-86.647462	-9.042042	1.741670
-87.208504	-4.183865	1.746675
-87.357403	-2.778117	1.751680
-87.238118	-13.027845	1.756685
-87.554793	-9.859137	1.761690
-88.340020	-10.809296	1.766694
-88.718964	-1.354231	1.771699
-88.601345	-16.194139	1.776704
-88.572930	-6.087521	1.781709
-88.693017	-9.757572	1.786714
-88.902044	-10.414646	1.791718
-89.509186	0.293951	1.796723
-89.965778	-11.742151	1.801728
-90.141923	-11.702016	1.806733
-90.322092	-3.720522	1.811738
-90.612735	-9.477328	1.816742
-91.387193	-13.855384	1.821747
-91.285270	-12.608908	1.826752
-91.861635	-2.974415	1.831757
-91.675060	-8.046252	1.836762
-91.585076	-11.388357	1.841766
-91.815028	-7.002496	1.846771
-92.107276	-6.121738	1.851776
-92.618825	-6.257163	1.856781
-93.182631	-8.997616	1.861786
-93.203850	-8.459604	1.866790
-93.627591	-3.565860	1.871795
-93.200133	-11.193459	1.876800
-93.543530	-14.382666	1.881805
-94.133029	-8.216641	1.886810
-94.457764	-2.604348	1.891814
-94.502340	-1.581825	1.896819
-94.888213	-10.990462	1.901824
-94.927416	-6.590010	1.906829
-95.737022	-14.689359	1.911834
-95.985374	-12.553145	1.916838
-96.336380	-4.794978	1.921843
-96.081372	-17.682164	1.926848
-96.172371	-11.780412	1.931853
-96.634085	-14.074870	1.936858
-96.243705	-15.299818	1.941862
-97.145107	-13.156831	1.946867
-97.428647	-12.125575	1.951872
-97.649933	-11.787357	1.956877
-97.668915	-6.947145	1.961882
-97.663557	-11.620619	1.966886
-98.527876	-4.763257	1.971891
-98.864698	-8.991163	1.976896
-99.010527	-11.565750	1.981901
-99.282566	-7.204973	1.986906
-99.030140	-19.003464	1.991910
-99.790372	-11.206893	1.996915
-100.197990	-14.625754	2.006912
-99.593020	-6.943166	2.016909
-99.295453	-6.770819	2.026906
-98.758074	-7.050779	2.036902
-97.972251	-7.363087	2.046899
-97.777856	-6.677349	2.056896
-97.234515	-10.727787	2.066893
-96.652341	-13.045211	2.076890
-96.498158	-12.723832	2.086886
-95.735936	-7.175407	2.096883
-95.197628	-1.579446	2.106880
-94.322064	-4.759816	2.116877
-94.645018	-2.843654	2.126874
-93.551883	-6.444358	2.136870
-92.794925	-8.025582	2.146867
-93.011778	-8.942017	2.156864
-92.147371	-10.147178	2.166861
-91.876484	-0.844562	2.176858
-91.080010	-4.937583	2.186854
-90.294987	-11.303221	2.196851
-90.088547	-12.510469	2.206848
-90.128122	-11.915009	2.216845
-89.197708	-10.308036	2.226842
-88.832004	-11.039587	2.236838
-87.882361	-16.268313	2.246835
-87.284906	-14.907261	2.256832
-87.596493	-11.209461	2.266829
-86.543030	-6.431783	2.276826
-86.198442	-3.713599	2.286822
-85.688848	-7.606735	2.296819
-84.942783	-17.023126	2.306816
-84.637823	-18.302731	2.316813
-84.224163	-14.309222	2.326810
-83.338986	-14.111163	2.336806
-83.318933	-7.937183	2.346803
-82.902684	-15.116516	2.356800
-82.002974	-15.468729	2.366797
-81.839981	-18.706036	2.376794
-80.993412	-11.137089	2.386790
-80.469175	-11.820466	2.396787
-80.178176	-12.705105	2.406784
-79.826000	-8.100160	2.416781
-79.136336	-8.292962	2.426778
-78.450442	-8.333127	2.436774
-77.574895	-2.324023	2.446771
-77.401197	-12.173968	2.456768
-77.359130	-6.304345	2.466765
-77.023815	-13.512258	2.476762
-76.162056	-10.668698	2.486758
-75.629355	-12.715500	2.496755
-74.871275	-12.861935	2.506752
-74.674415	-12.664405	2.516749
-74.208285	-14.121155	2.526746
-73.346017	-4.875773	2.536742
-73.152703	-9.156805	2.546739
-72.904234	-9.832090	2.556736
-72.274498	-13.249771	2.566733
-71.361522	-12.064553	2.576730
-70.762422	-13.032007	2.586726
-70.369807	-12.326449	2.596723
-70.143841	-9.783025	2.606720
-70.033581	-12.340573	2.616717
-69.025124	-16.377901	2.626714
-68.652993	-12.846743	2.636710
-68.001728	-9.998919	2.646707
-67.279203	-13.991728	2.656704
-67.387154	-10.718428	2.666701
-66.656764	-15.434695	2.676698
-66.001771	-13.705645	2.686694
-65.590588	-16.892900	2.696691
-64.477727	-11.817204	2.706688
-64.484618	-15.731288	2.716685
-64.384403	-14.695111	2.726682
-63.632310	-12.639070	2.736678
-63.048121	-13.100540	2.746675
-62.774781	-8.407295	2.756672
-61.893598	-10.847299	2.766669
-61.432236	-12.778459	2.776666
-61.414174	-6.046654	2.786662
-60.698393	-16.329446	2.796659
-60.055432	-7.319172	2.806656
-59.418203	-13.205651	2.816653
-58.527625	-6.004668	2.826650
-58.454510	0.794593	2.836646
-58.413999	-12.721809	2.846643
-57.419553	-3.509676	2.856640
-57.160235	-9.445017	2.866637
-56.806145	-4.618629	2.876634
-55.656242	-1.610864	2.886630
-55.471383	-3.093509	2.896627
-55.359186	-10.257181	2.906624
-54.817193	-5.263654	2.916621
-54.161131	-9.128912	2.926618
-53.266796	-7.462468	2.936614
-52.527967	-5.369515	2.946611
-52.817963	-5.311585	2.956608
-52.436194	-6.954764	2.966605
-51.550515	-8.109385	2.976602
-51.265338	-15.803651	2.986598
-50.369295	-14.203995	2.996595
-50.247082	-16.209058	3.006592
-49.408237	-17.026947	3.016589
-48.904365	-11.853262	3.026586
-48.690643	-9.314266	3.036582
-48.002343	-14.163359	3.046579
-47.362666	-13.398070	3.056576
-47.100508	-16.090136	3.066573
-46.830199	-19.543717	3.076570
-46.024310	-11.867066	3.086566
-45.664499	-14.153035	3.096563
-44.711909	-7.484375	3.106560
-44.358626	-12.141928	3.116557
-44.354066	-14.093828	3.126554
-43.370442	-11.386445	3.136550
-43.185099	-9.739487	3.146547
-42.629144	-5.913843	3.156544
-41.754207	-9.287343	3.166541
-41.551672	-3.651770	3.176538
-40.854769	-12.471320	3.186534
-40.016947	-10.732723	3.196531
-39.871700	-7.451329	3.206528
-39.769864	-6.418571	3.216525
-39.203482	-9.706017	3.226522
-38.457458	-14.605277	3.236518
-38.311253	-12.274340	3.246515
-37.123453	-12.703084	3.256512
-36.768271	-19.096825	3.266509
-36.881942	-18.673555	3.276506
-35.868443	-16.474487	3.286502
-35.434804	-11.068128	3.296499
-35.183039	-19.096134	3.306496
-34.332334	-11.882607	3.316493
-34.166918	-9.272736	3.326490
-33.803966	-13.187387	3.336486
-32.846692	-10.729317	3.346483
-32.592794	-11.652526	3.356480
-31.883188	-11.408122	3.366477
-31.404978	-13.234204	3.376474
-31.127616	-8.132952	3.386470
-30.355793	-5.722031	3.396467
-29.713212	-8.501839	3.406464
-29.387031	-6.493518	3.416461
-29.071198	-11.658407	3.426458
-28.224988	-10.833410	3.436454
-28.127714	-7.202435	3.446451
-27.694971	-18.511839	3.456448
-26.950090	-11.817175	3.466445
-26.612140	-13.615083	3.476442
-25.936768	-8.312881	3.486438
-25.172939	-3.914572	3.496435
-24.802147	-9.433297	3.506432
-24.683854	-18.036049	3.516429
-23.722698	-14.891194	3.526426
-23.576057	-12.443120	3.536422
-23.405105	-12.311245	3.546419
-22.329388	-12.529308	3.556416
-21.988207	-17.555595	3.566413
-21.293864	-12.645974	3.576410
-20.712173	-11.605569	3.586406
-20.577324	-9.152491	3.596403
-20.216673	-19.883653	3.606400
-19.526868	-14.032522	3.616397
-18.981170	-18.818231	3.626394
-17.898202	-15.049300	3.636390
-17.524531	-14.077873	3.646387
-17.436125	-19.067972	3.656384
-17.538752	-21.462497	3.666381
-16.787742	-14.296801	3.676378
-15.946701	-17.820238	3.686374
-15.081421	-18.144915	3.696371
-14.745614	-15.615424	3.706368
-14.737995	-21.109277	3.716365
-14.271762	-19.585246	3.726362
-13.694339	-13.396680	3.736358
-12.486862	-13.533891	3.746355
-12.142007	-15.367719	3.756352
-12.081292	-15.570293	3.766349
-11.652633	-19.282939	3.776346
-10.774015	-15.371322	3.786342
-10.505834	-6.641632	3.796339
-10.035470	-14.215853	3.806336
-8.944444	-15.529152	3.816333
-8.561677	-13.418772	3.826330
-8.560225	-17.726950	3.836326
-8.395451	-16.361881	3.846323
-7.173919	-11.094032	3.856320
-7.047026	-18.652785	3.866317
-6.628221	-17.644038	3.876314
-6.376681	-7.565489	3.886310
-5.481418	-4.521241	3.896307
-5.453637	-8.317187	3.906304
-4.917508	9.759834	3.916301
-4.224450	27.441820	3.926298
-3.674746	29.738449	3.936294
-3.098950	42.462253	3.946291
-2.622661	43.870687	3.956288
-2.045790	51.877624	3.966285
-1.820302	58.111508	3.976282
-1.338664	76.916151	3.986278
-0.974150	91.120529	3.996275
-0.402484	100.756501	4.006272
0.000000	122.883373	4.011277
0.082633	125.335057	4.016282
-0.301731	134.575913	4.021286
0.034569	138.905285	4.026291
0.148192	149.397355	4.031296
0.264118	148.218292	4.036301
0.840148	156.822425	4.041306
1.061731	162.106110	4.046310
1.230167	159.764131	4.051315
1.094187	161.961963	4.056320
1.071173	152.578989	4.061325
0.881925	150.175646	4.066330
0.570679	158.361120	4.071334
1.015005	161.205734	4.076339
0.619637	157.761998	4.081344
1.237563	172.512956	4.086349
1.256045	170.716330	4.091354
1.059829	156.981797	4.096358
1.011550	150.589263	4.101363
0.886374	156.233812	4.106368
0.650560	154.027539	4.111373
1.260044	159.753852	4.116378
1.238945	171.165393	4.121382
1.377678	160.561363	4.126387
0.862399	161.388271	4.131392
1.084563	155.447161	4.136397
1.046666	156.984331	4.141402
0.979708	170.177831	4.146406
1.408823	169.826342	4.151411
0.827748	176.332798	4.156416
0.798618	171.044562	4.161421
1.572401	168.946844	4.166426
1.177314	177.787606	4.171430
1.234280	172.258179	4.176435
1.207269	173.651291	4.181440
1.506114	172.595604	4.186445
1.417817	163.153188	4.191450
1.394969	157.933577	4.196454
1.307842	148.937064	4.201459
1.171880	158.379697	4.206464
0.791383	153.671341	4.211469
0.981955	159.307858	4.216474
1.506082	170.435197	4.221478
1.782301	176.729083	4.226483
1.480265	170.132448	4.231488
1.182433	168.619183	4.236493
1.515314	164.587508	4.241498
0.982263	168.194888	4.246502
1.173751	171.142144	4.251507
1.218076	167.123759	4.256512
1.269797	178.723278	4.261517
1.479964	178.788684	4.266522
1.494988	181.124354	4.271526
1.906773	183.743090	4.276531
1.452856	173.408492	4.281536
1.665408	171.701869	4.286541
1.732120	177.515860	4.291546
1.325625	176.193514	4.296550
1.457128	166.346724	4.301555
1.325562	171.065317	4.306560
1.649911	183.027342	4.311565
1.703423	181.193623	4.316570
1.542444	181.781875	4.321574
1.565390	181.977668	4.326579
1.695089	188.158332	4.331584
1.406791	184.922542	4.336589
1.645438	182.632902	4.341594
1.362457	184.394891	4.346598
1.705468	189.868481	4.351603
1.696908	186.908666	4.356608
1.583920	184.879414	4.361613
1.976713	181.369905	4.366618
1.633594	176.851871	4.371622
2.132617	181.016717	4.376627
1.695893	175.266770	4.381632
1.171086	172.877705	4.386637
1.393538	183.919149	4.391642
1.610976	183.790438	4.396646
1.600486	182.333670	4.401651
1.682182	189.872699	4.406656
1.827155	183.494356	4.411661
2.015106	188.590301	4.416666
1.455280	192.211345	4.421670
1.818501	182.534107	4.426675
1.808848	185.829050	4.431680
1.442228	189.983147	4.436685
1.678956	184.678822	4.441690
1.629342	193.589186	4.446694
1.924167	181.730169	4.451699
1.741874	191.540692	4.456704
1.568156	183.345399	4.461709
1.972084	195.469044	4.466714
1.989085	206.485544	4.471718
2.375285	202.031117	4.476723
2.089642	192.625739	4.481728
1.788487	189.404603	4.486733
1.830650	187.357521	4.491738
1.940727	189.953633	4.496742
2.040478	193.718750	4.501747
1.697234	193.946248	4.506752
2.143359	198.979854	4.511757
2.385644	200.122236	4.516762
2.008040	206.755207	4.521766
2.060086	189.438675	4.526771
1.751396	190.796553	4.531776
2.328973	198.884786	4.536781
2.487184	201.147546	4.541786
1.807061	196.318156	4.546790
2.110035	199.640354	4.551795
2.420703	212.199301	4.556800
2.341673	209.063797	4.561805
2.061656	186.692790	4.566810
1.330713	188.644746	4.571814
2.135458	196.365422	4.576819
1.997249	203.448325	4.581824
1.984529	203.026426	4.586829
2.259424	206.830714	4.591834
2.024235	206.155558	4.596838
2.479343	211.855305	4.601843
2.247576	208.189939	4.606848
2.118401	210.481627	4.611853
2.503249	213.227946	4.616858
2.302675	211.633096	4.621862
2.328916	202.669524	4.626867
2.424393	202.774932	4.631872
2.353088	201.106174	4.636877
2.417777	201.545399	4.641882
2.330388	207.203062	4.646886
2.482866	198.235656	4.651891
2.162491	200.905117	4.656896
2.188031	202.552634	4.661901
2.443438	206.144826	4.666906
2.321015	199.428468	4.671910
2.516365	201.935377	4.676915
2.272768	206.298107	4.681920
2.248947	199.170938	4.686925
2.619125	194.212819	4.691930
2.136585	205.572844	4.696934
2.654642	196.725684	4.701939
2.392015	201.888623	4.706944
2.081141	221.102656	4.711949
2.569544	221.884024	4.716954
2.666455	233.255085	4.721958
3.110138	222.834487	4.726963
2.711215	216.426923	4.731968
2.403903	213.526273	4.736973
2.680414	205.320981	4.741978
2.541400	210.372930	4.746982
2.579177	196.753791	4.751987
2.619944	214.628613	4.756992
2.575343	215.869447	4.761997
2.706768	221.597448	4.767002
2.805338	224.296594	4.772006
2.809171	217.108166	4.777011
2.909330	215.346273	4.782016
2.234759	217.397020	4.787021
2.571984	208.321751	4.792026
2.361647	223.897720	4.797030
2.865426	224.762114	4.802035
3.087340	227.891300	4.807040
2.813849	226.086345	4.812045
3.251440	230.203820	4.817050
3.051363	230.184406	4.822054
2.650250	211.239510	4.827059
3.014601	206.374042	4.832064
2.547975	216.526234	4.837069
2.735529	211.283340	4.842074
2.717478	224.735015	4.847078
2.655443	231.935780	4.852083
3.034484	231.952747	4.857088
3.080581	232.100644	4.862093
2.855631	220.797082	4.867098
2.834036	230.630061	4.872102
2.666846	235.714877	4.877107
2.983626	225.987900	4.882112
3.054330	228.530038	4.887117
3.206268	227.282090	4.892122
3.025459	240.116889	4.897126
3.248332	235.118421	4.902131
3.145019	233.008564	4.907136
3.120234	231.019356	4.912141
3.097975	228.049013	4.917146
2.740605	221.407192	4.922150
3.052953	220.115287	4.927155
2.932857	229.729489	4.932160
3.032709	227.296942	4.937165
3.210923	229.385753	4.942170
3.130499	232.891036	4.947174
3.125262	229.282142	4.952179
3.159805	224.914098	4.957184
2.725531	235.032790	4.962189
3.393642	225.017000	4.967194
3.184025	232.297689	4.972198
3.447925	224.477157	4.977203
3.236428	226.952504	4.982208
3.186110	235.129024	4.987213
3.270955	222.666773	4.992218
3.008679	232.050019	4.997222
3.164775	217.773378	5.002227
3.246478	231.294946	5.007232
2.956491	231.004799	5.012237
3.116254	223.526341	5.017242
3.101623	228.426054	5.022246
3.051280	225.947291	5.027251
3.340383	225.108248	5.032256
2.911599	231.524575	5.037261
3.201930	239.578458	5.042266
3.508088	259.449419	5.047270
3.536205	251.874389	5.052275
4.054976	241.606600	5.057280
3.437952	234.767925	5.062285
3.343113	233.912732	5.067290
3.058487	244.954071	5.072294
3.142157	231.628311	5.077299
3.618684	250.384428	5.082304
3.504173	256.751832	5.087309
3.641812	242.772268	5.092314
3.117633	241.901666	5.097318
3.344523	248.139984	5.102323
3.734097	255.359027	5.107328
3.695711	257.231634	5.112333
3.707077	254.891952	5.117338
3.820819	253.159578	5.122342
3.347686	236.279102	5.127347
3.547345	246.656595	5.132352
3.561732	257.977248	5.137357
3.796355	240.398126	5.142362
3.517238	253.912616	5.147366
3.608374	250.924614	5.152371
3.519769	247.664047	5.157376
3.479589	250.555639	5.162381
3.882324	254.365342	5.167386
3.807721	258.005762	5.172390
3.837148	254.021314	5.177395
3.780129	248.190079	5.182400
3.663454	250.106511	5.187405
3.831076	253.465612	5.192410
3.682895	258.860680	5.197414
3.786506	260.689033	5.202419
3.785237	258.993547	5.207424
3.593543	251.841875	5.212429
3.552302	250.642985	5.217434
3.628211	259.480056	5.222438
3.467000	262.884030	5.227443
3.710261	267.645526	5.232448
3.435100	265.110014	5.237453
3.684150	256.152852	5.242458
3.535542	258.763941	5.247462
3.812521	257.332011	5.252467
3.957271	257.398111	5.257472
3.903323	257.204088	5.262477
3.629061	249.872287	5.267482
3.275429	263.376240	5.272486
3.966097	265.426395	5.277491
4.167149	269.808494	5.282496
4.343362	276.329953	5.287501
4.233471	274.739961	5.292506
4.103521	277.721464	5.297510
3.831396	272.540632	5.302515
3.831280	277.317878	5.307520
3.981802	274.190914	5.312525
4.219782	283.091346	5.317530
4.029084	284.225220	5.322534
4.144850	284.014264	5.327539
4.138141	280.563774	5.332544
4.113898	285.629511	5.337549
4.284201	279.130133	5.342554
4.292478	272.475655	5.347558
4.131912	266.666862	5.352563
3.841903	264.487996	5.357568
3.731942	274.603671	5.362573
3.865225	278.543915	5.367578
3.998636	290.152934	5.372582
4.294674	279.299719	5.377587
4.066344	284.175774	5.382592
4.196962	281.883959	5.387597
4.296500	279.223668	5.392602
3.999876	280.209522	5.397606
4.149225	282.856479	5.402611
4.164302	278.662293	5.407616
3.759629	283.107068	5.412621
4.073544	280.827842	5.417626
3.863182	302.231406	5.422630
4.363937	303.156386	5.427635
4.486340	308.730799	5.432640
4.658232	305.050019	5.437645
4.565013	293.029887	5.442650
4.076985	298.867015	5.447654
4.535399	297.963643	5.452659
4.328822	300.447725	5.457664
4.625640	308.807508	5.462669
4.709530	290.546301	5.467674
4.295147	294.280759	5.472678
4.309336	291.649573	5.477683
4.386296	293.029670	5.482688
4.223015	308.497148	5.487693
4.438446	305.106977	5.492698
4.644348	312.851342	5.497702
4.539813	299.051806	5.502707
4.791681	309.085855	5.507712
4.449585	303.583720	5.512717
4.700312	301.981870	5.517722
4.429782	306.883483	5.522726
4.633150	307.706072	5.527731
4.513246	301.302489	5.532736
4.486242	313.173777	5.537741
4.742210	308.799711	5.542746
4.731003	304.280586	5.547750
4.746814	311.039000	5.552755
4.849695	302.335522	5.557760
4.905606	303.415183	5.562765
4.526954	290.506203	5.567770
4.273492	293.393045	5.572774
4.724669	302.469097	5.577779
4.973826	308.289525	5.582784
4.735991	301.765101	5.587789
4.361833	302.354912	5.592794
4.606387	303.889246	5.597798
4.812635	313.085694	5.602803
4.915003	313.759496	5.607808
4.886503	311.919551	5.612813
4.949193	306.294280	5.617818
5.006703	308.670808	5.622822
4.881974	295.643197	5.627827
4.615748	291.508624	5.632832
4.679337	303.356309	5.637837
4.822107	297.962178	5.642842
4.638791	306.387224	5.647846
5.053571	306.455573	5.652851
5.281041	299.118398	5.657856
4.864646	307.089362	5.662861
5.005830	293.087060	5.667866
5.147344	310.547668	5.672870
5.095088	294.547553	5.677875
4.896696	292.009575	5.682880
4.954771	291.972114	5.687885
4.868177	292.184963	5.692890
4.836162	300.374482	5.697894
4.679861	303.379073	5.702899
5.315934	308.414773	5.707904
5.074247	312.163475	5.712909
5.131526	299.800372	5.717914
4.971627	309.999772	5.722918
4.975395	310.435829	5.727923
5.024245	312.788396	5.732928
4.860892	312.981560	5.737933
4.894563	306.503445	5.742938
4.954811	319.895546	5.747942
4.965930	316.549838	5.752947
4.612936	322.777230	5.757952
4.682863	317.666512	5.762957
4.968933	311.762856	5.767962
4.937826	328.842241	5.772966
5.215534	333.452861	5.777971
5.612027	334.337129	5.782976
5.118777	339.263937	5.787981
5.547421	336.447994	5.792986
5.577605	327.951973	5.797990
5.627481	322.898158	5.802995
5.408838	316.104990	5.808000
4.919367	311.549599	5.813005
5.039085	310.714779	5.818010
5.070820	323.529201	5.823014
4.930360	333.823662	5.828019
5.190717	332.020997	5.833024
5.643228	344.001141	5.838029
5.502577	338.616324	5.843034
5.534037	338.276127	5.848038
5.689710	335.556468	5.853043
5.732143	323.119733	5.858048
5.266136	317.886818	5.863053
5.243690	309.079466	5.868058
5.174147	315.234250	5.873062
5.320026	322.250822	5.878067
5.694527	332.642272	5.883072
5.535529	343.822298	5.888077
5.664476	333.311436	5.893082
5.878275	333.831850	5.898086
5.586810	313.787786	5.903091
5.659901	309.416883	5.908096
5.560909	317.936372	5.913101
5.267219	307.054738	5.918106
5.270038	316.456865	5.923110
5.185799	331.658960	5.928115
5.683165	332.518031	5.933120
5.517046	335.242587	5.938125
5.846128	329.828929	5.943130
5.692613	335.183723	5.948134
5.699139	336.742466	5.953139
5.594683	335.417373	5.958144
5.511687	333.785224	5.963149
5.514032	336.426604	5.968154
5.761494	336.432421	5.973158
5.579433	332.708670	5.978163
5.943034	334.920487	5.983168
5.519366	343.942948	5.988173
5.593506	342.400226	5.993178
5.637494	336.059698	5.998182
5.790032	330.831712	6.003187
5.907573	334.565615	6.008192
5.506878	342.398111	6.013197
5.800987	336.050276	6.018202
5.801852	347.860301	6.023206
5.697604	341.194843	6.028211
5.692278	342.258730	6.033216
5.249457	339.907497	6.038221
5.461736	343.895567	6.043226
5.675216	339.271849	6.048230
5.529636	336.678187	6.053235
5.763352	340.191526	6.058240
5.539960	352.748304	6.063245
5.787048	357.784471	6.068250
5.933179	363.655759	6.073254
5.916656	358.419287	6.078259
5.608235	356.015488	6.083264
5.399415	352.273754	6.088269
5.639567	356.406181	6.093274
5.612151	361.820442	6.098278
5.872193	369.429853	6.103283
5.857918	362.911728	6.108288
6.076416	357.458332	6.113293
5.937235	358.770848	6.118298
5.570053	355.253083	6.123302
5.806629	360.328853	6.128307
5.531377	366.107564	6.133312
5.908788	366.823964	6.138317
6.235220	356.649331	6.143322
5.917769	362.238461	6.148326
6.087147	358.662464	6.153331
5.825157	342.198260	6.158336
5.851565	343.823509	6.163341
5.833394	336.957992	6.168346
5.679274	342.452085	6.173350
5.633850	345.765282	6.178355
5.518148	344.233135	6.183360
5.602928	363.167423	6.188365
5.845888	365.110129	6.193370
5.814236	367.218977	6.198374
5.899098	362.646915	6.203379
5.832446	362.375777	6.208384
5.719528	369.837616	6.213389
5.741611	362.766508	6.218394
5.356689	364.965160	6.223398
5.693213	361.157497	6.228403
5.756516	355.161962	6.233408
5.766464	358.014130	6.238413
6.056580	361.793935	6.243418
5.941452	357.186575	6.248422
5.780341	367.240665	6.253427
6.277625	364.410868	6.258432
5.649053	367.378271	6.263437
5.881676	361.299425	6.268442
5.894536	361.968182	6.273446
5.777870	352.514264	6.278451
5.779014	348.347540	6.283456
5.702583	346.005698	6.288461
5.813104	347.291990	6.293466
5.802499	360.413583	6.298470
5.834731	359.598709	6.303475
5.982750	350.347187	6.308480
5.642279	343.943130	6.313485
5.789243	341.297592	6.318490
5.768839	342.752962	6.323494
5.599051	341.036251	6.328499
5.656823	347.174387	6.333504
5.884658	363.735769	6.338509
5.596953	358.228312	6.343514
5.853517	365.085301	6.348518
5.803909	365.630909	6.353523
6.513349	357.994046	6.358528
5.725862	353.295221	6.363533
5.945296	343.614974	6.368538
5.573524	338.784990	6.373542
5.555637	336.706112	6.378547
5.518479	352.824696	6.383552
5.654842	366.239781	6.388557
5.642247	364.498593	6.393562
5.973152	371.071931	6.398566
5.822699	376.511680	6.403571
6.044905	356.792546	6.408576
5.883800	368.545547	6.413581
6.019814	350.111650	6.418586
5.437359	357.637099	6.423590
5.691510	354.971706	6.428595
5.827083	365.469977	6.433600
5.707593	370.658135	6.438605
5.874490	363.479059	6.443610
5.609879	367.889393	6.448614
5.861401	368.125528	6.453619
5.944767	361.620674	6.458624
5.628204	366.507324	6.463629
6.038350	367.281902	6.468634
5.914441	369.528499	6.473638
5.411949	365.528770	6.478643
5.522100	361.772171	6.483648
5.758518	371.017735	6.488653
6.100947	370.176710	6.493658
5.759231	374.614868	6.498662
5.775158	370.863447	6.503667
6.112192	368.821053	6.508672
5.370142	364.260682	6.513677
5.825661	365.512242	6.518682
5.980573	366.671404	6.523686
5.749318	371.396079	6.528691
5.916862	358.854419	6.533696
5.606473	370.450333	6.538701
5.759214	363.956822	6.543706
5.590004	363.227095	6.548710
5.627004	367.438611	6.553715
5.814345	363.698467	6.558720
5.808058	367.328272	6.563725
5.674437	362.445384	6.568730
5.886302	369.189113	6.573734
5.728710	366.208181	6.578739
5.711226	365.891422	6.583744
5.650689	378.445008	6.588749
5.778144	361.281080	6.593754
6.086585	370.812818	6.598758
5.713023	374.272022	6.603763
5.844924	365.348863	6.608768
6.049286	369.752617	6.613773
5.514233	363.204846	6.618778
5.788426	371.207518	6.623782
6.056163	363.854556	6.628787
6.155910	365.275403	6.633792
6.002782	368.570573	6.638797
5.749873	357.287095	6.643802
5.690719	353.155068	6.648806
5.727507	353.506893	6.653811
5.697564	356.694297	6.658816
6.037975	359.890476	6.663821
5.737735	353.113162	6.668826
5.848027	358.069390	6.673830
5.981415	359.019934	6.678835
5.874092	343.085296	6.683840
5.493179	353.967691	6.688845
5.674146	338.563965	6.693850
5.574029	352.544198	6.698854
5.447439	370.859679	6.703859
5.788708	371.053368	6.708864
5.776050	369.223605	6.713869
5.991319	366.159310	6.718874
6.033818	370.509173	6.723878
5.958079	366.569548	6.728883
6.165759	356.628536	6.733888
5.812874	345.072734	6.738893
5.844111	339.825668	6.743898
5.307096	345.341413	6.748902
5.636534	352.063666	6.753907
5.809835	354.988475	6.758912
5.852758	369.196382	6.763917
5.430561	373.991916	6.768922
5.793022	373.774186	6.773926
5.607581	371.028540	6.778931
5.956810	367.721927	6.783936
5.705159	363.344626	6.788941
5.546642	369.067199	6.793946
5.575399	367.278444	6.798950
5.588426	363.758426	6.803955
5.707984	370.526019	6.808960
5.138814	366.473397	6.813965
5.900371	360.596931	6.818970
5.930078	361.835696	6.823974
5.660109	366.468323	6.828979
6.082685	361.657022	6.833984
6.247657	371.391429	6.838989
6.138880	374.638567	6.843994
6.045360	367.072935	6.848998
5.914180	368.871417	6.854003
6.040174	360.199114	6.859008
5.889552	373.257096	6.864013
5.898362	367.035927	6.869018
5.808277	363.949573	6.874022
5.385935	363.040963	6.879027
5.606602	356.248982	6.884032
5.598552	365.972361	6.889037
5.860130	366.656177	6.894042
6.025986	371.195638	6.899046
5.916983	369.327093	6.904051
6.174018	369.245999	6.909056
5.869021	360.634472	6.914061
5.633355	356.836806	6.919066
5.703793	353.061083	6.924070
5.494425	371.402109	6.929075
5.678947	373.085000	6.934080
6.211152	365.083428	6.939085
5.950637	363.228983	6.944090
5.780145	359.066834	6.949094
5.402617	353.756858	6.954099
5.798074	362.281640	6.959104
5.673791	375.768951	6.964109
5.700781	366.381242	6.969114
6.040457	375.114029	6.974118
5.733962	375.493992	6.979123
5.939947	369.371835	6.984128
6.057177	368.803151	6.989133
5.926931	363.381907	6.994138
5.883216	358.137013	6.999142
5.862988	356.884225	7.004147
5.808918	348.581643	7.009152
5.764823	343.884134	7.014157
5.872960	346.081944	7.019162
5.651459	346.717589	7.024166
5.285777	346.198784	7.029171
5.558220	357.912748	7.034176
5.707892	361.629000	7.039181
5.915780	366.475124	7.044186
6.037550	364.535848	7.049190
6.012151	367.200534	7.054195
6.009725	355.827439	7.059200
5.515649	363.263201	7.064205
5.731745	347.195947	7.069210
5.777479	362.634093	7.074214
5.825488	358.317703	7.079219
6.012998	360.664506	7.084224
5.721290	366.376178	7.089229
5.738085	359.603283	7.094234
5.642734	352.487189	7.099238
5.787809	351.477579	7.104243
5.907330	359.817535	7.109248
6.034439	356.409469	7.114253
5.727543	351.382722	7.119258
5.530524	352.305616	7.124262
5.623407	355.034141	7.129267
6.094985	358.646489	7.134272
5.726183	349.801296	7.139277
5.832670	345.450495	7.144282
6.101623	349.372795	7.149286
5.626444	350.705988	7.154291
5.908244	349.703564	7.159296
5.774526	352.296529	7.164301
5.622162	353.421275	7.169306
5.518014	351.479211	7.174310
5.399341	360.814857	7.179315
5.637024	366.244790	7.184320
5.511519	369.757119	7.189325
5.795502	362.461739	7.194330
5.904556	369.680213	7.199334
5.851098	369.574697	7.204339
6.187515	367.908880	7.209344
5.455920	373.916831	7.214349
5.589262	378.170295	7.219354
5.710097	375.316852	7.224358
5.755669	378.229914	7.229363
6.080934	366.533712	7.234368
5.781999	377.491942	7.239373
5.578775	373.265284	7.244378
5.777494	370.111817	7.249382
5.880806	369.754105	7.254387
5.831871	369.382133	7.259392
5.711804	372.941071	7.264397
5.699379	370.215942	7.269402
5.957945	370.925537	7.274406
6.070699	364.748296	7.279411
5.916670	368.347321	7.284416
5.606679	379.788157	7.289421
5.505529	371.423293	7.294426
5.813806	373.143862	7.299430
5.577130	374.579126	7.304435
6.190415	372.088765	7.309440
5.719664	373.987573	7.314445
6.087067	370.738241	7.319450
6.028711	376.574934	7.324454
6.045973	383.643192	7.329459
6.020391	371.043009	7.334464
5.615682	362.918398	7.339469
5.616612	354.683179	7.344474
5.836685	358.929463	7.349478
5.642092	357.143847	7.354483
5.865749	362.357667	7.359488
5.604544	370.022926	7.364493
6.175203	374.837879	7.369498
5.989159	362.376579	7.374502
5.244783	358.401857	7.379507
5.492401	364.304799	7.384512
5.612908	373.242549	7.389517
5.742575	369.641096	7.394522
5.787984	371.810711	7.399526
5.863540	375.143042	7.404531
5.967299	375.819793	7.409536
5.742762	377.816307	7.414541
5.908825	378.087894	7.419546
6.172505	384.630575	7.424550
5.756370	373.875531	7.429555
5.955885	381.121054	7.434560
5.815942	374.749038	7.439565
6.219637	364.015049	7.444570
5.740491	354.437236	7.449574
5.528204	359.772714	7.454579
5.965535	348.362791	7.459584
5.336548	359.014899	7.464589
5.410229	366.311645	7.469594
5.622114	375.798308	7.474598
5.621920	382.230215	7.479603
5.636006	376.593508	7.484608
5.675559	378.909567	7.489613
5.965482	374.511216	7.494618
6.122429	373.740198	7.499622
5.729499	375.892642	7.504627
6.125257	369.895959	7.509632
5.859199	381.912078	7.514637
5.823212	374.489344	7.519642
6.139543	377.875935	7.524646
5.436621	376.862314	7.529651
5.601137	372.945391	7.534656
5.622185	378.010430	7.539661
5.536094	376.571745	7.544666
5.851837	380.493095	7.549670
5.705655	378.247529	7.554675
5.881271	382.111604	7.559680
5.942514	382.804466	7.564685
5.595251	386.348161	7.569690
5.489575	379.967645	7.574694
5.783108	379.482241	7.579699
5.906352	373.309690	7.584704
5.651826	374.896427	7.589709
5.868016	375.131736	7.594714
5.875865	375.329882	7.599718
5.733475	381.347336	7.604723
6.213936	380.684133	7.609728
5.492308	380.249221	7.614733
5.672608	376.456387	7.619738
5.868270	373.635585	7.624742
5.618079	374.475012	7.629747
5.810182	372.559585	7.634752
5.638611	376.980744	7.639757
5.769543	377.488752	7.644762
6.224087	383.261408	7.649766
6.071090	379.656507	7.654771
6.089274	375.458650	7.659776
5.969685	368.422252	7.664781
5.806024	370.513689	7.669786
6.007135	366.644853	7.674790
5.790350	366.412908	7.679795
5.770990	357.858148	7.684800
5.834972	360.996128	7.689805
5.642944	351.082552	7.694810
5.730554	352.150952	7.699814
5.720077	372.938194	7.704819
5.877808	375.954015	7.709824
5.796227	380.272580	7.714829
5.870722	370.096036	7.719834
5.702792	356.312654	7.724838
5.597958	367.949326	7.729843
6.004599	374.662732	7.734848
5.868092	373.412228	7.739853
5.515765	367.595295	7.744858
5.975458	367.780036	7.749862
5.742330	381.818966	7.754867
5.998318	373.553517	7.759872
5.976204	374.145464	7.764877
5.715150	364.375503	7.769882
5.720072	361.432543	7.774886
5.581255	360.732885	7.779891
5.846382	364.168573	7.784896
5.759387	372.461597	7.789901
5.642508	369.430033	7.794906
5.979312	373.841641	7.799910
5.516543	367.273122	7.804915
5.920407	374.186273	7.809920
5.875024	377.847477	7.814925
5.888564	380.366900	7.819930
6.126413	361.910809	7.824934
5.484904	357.989673	7.829939
5.514074	358.374321	7.834944
5.364528	371.422643	7.839949
5.475890	373.167544	7.844954
5.814245	377.047408	7.849958
5.597103	391.877947	7.854963
5.650816	381.293350	7.859968
5.935747	385.377684	7.864973
5.783422	381.285466	7.869978
6.359200	377.149488	7.874982
5.777470	374.658528	7.879987
5.843951	371.516159	7.884992
6.074150	375.210385	7.889997
5.991200	368.348614	7.895002
6.022878	364.787728	7.900006
5.855385	362.763778	7.905011
5.590873	353.057636	7.910016
5.440458	358.209476	7.915021
5.695044	380.369634	7.920026
6.117281	381.803546	7.925030
5.642688	380.893579	7.930035
6.218114	365.039277	7.935040
5.864221	361.712428	7.940045
5.945782	351.534795	7.945050
5.748897	345.339332	7.950054
5.936206	346.373227	7.955059
5.723919	347.640178	7.960064
5.821430	355.673517	7.965069
5.735585	354.601785	7.970074
5.685123	356.640795	7.975078
5.555328	355.028585	7.980083
5.912053	355.574202	7.985088
6.213516	356.362538	7.990093
5.964344	348.738892	7.995098
5.778160	353.690660	8.000102
5.732171	354.279996	8.005107
5.864011	346.546409	8.010112
5.937583	345.879476	8.015130
5.592514	359.616089	8.020147
5.699492	354.821854	8.025165
5.619277	356.390126	8.030182
5.432071	352.364336	8.035200
5.546614	352.731543	8.040218
5.644709	375.102412	8.045235
5.923262	375.958453	8.050253
5.617134	383.794289	8.055270
6.098809	375.265389	8.060288
5.899754	380.840894	8.065306
5.573780	378.600707	8.070323
5.765621	369.403761	8.075341
5.906696	379.716567	8.080358
6.032376	375.967088	8.085376
5.924267	374.797454	8.090394
6.188088	373.506798	8.095411
6.126939	363.642383	8.100429
5.570670	356.568908	8.105446
5.794962	363.208211	8.110464
5.615428	368.828007	8.115482
5.682620	379.527837	8.120499
5.836818	377.266534	8.125517
5.377051	388.007392	8.130534
5.791029	384.579078	8.135552
5.884135	376.984788	8.140570
5.777196	383.088722	8.145587
5.962901	376.123766	8.150605
5.809902	382.714527	8.155622
6.172039	369.123662	8.160640
5.974086	370.786002	8.165658
5.639811	375.322263	8.170675
5.299499	367.584032	8.175693
5.697034	383.158382	8.180710
6.121007	388.576928	8.185728
5.882979	389.008497	8.190746
5.944813	392.056741	8.195763
5.962811	384.521477	8.200781
5.972538	395.877170	8.205798
6.449002	385.812279	8.210816
5.740768	384.060775	8.215834
5.933324	370.228083	8.220851
6.129917	375.022499	8.225869
6.246736	385.149746	8.230886
5.829034	378.187225	8.235904
6.162548	375.920093	8.240922
5.941339	379.880204	8.245939
6.049115	374.344264	8.250957
5.982037	379.968644	8.255974
5.915725	371.673381	8.260992
5.963321	372.439156	8.266010
5.780299	394.434118	8.271027
6.078800	389.569031	8.276045
5.928254	405.777817	8.281062
5.847735	394.710944	8.286080
6.216359	401.895805	8.291098
6.075540	404.631638	8.296115
6.428289	394.652272	8.301133
6.311774	391.925058	8.306150
6.342741	395.618703	8.311168
5.926192	387.844999	8.316186
6.148037	394.251177	8.321203
6.440189	386.922523	8.326221
6.148851	380.767104	8.331238
5.692093	372.034041	8.336256
6.177249	376.622591	8.341274
6.245924	384.355893	8.346291
6.097565	384.656742	8.351309
6.008956	377.807076	8.356326
6.229767	388.205297	8.361344
5.905122	386.296244	8.366362
5.981302	396.963129	8.371379
6.435692	396.870346	8.376397
6.094140	410.619073	8.381414
6.350585	401.225870	8.386432
6.158470	400.823512	8.391450
5.955960	404.550355	8.396467
6.193656	398.479810	8.401485
6.333908	402.964286	8.406502
6.319844	409.145281	8.411520
6.359483	398.056542	8.416538
6.323862	396.301294	8.421555
6.218396	382.584417	8.426573
5.947372	382.793918	8.431590
6.423639	387.219762	8.436608
6.496179	381.670372	8.441626
6.233007	383.049393	8.446643
6.216518	378.700387	8.451661
6.393887	380.506252	8.456678
6.105259	371.709144	8.461696
6.056732	371.416968	8.466714
5.774333	385.620345	8.471731
6.272777	389.477877	8.476749
6.539713	400.541075	8.481766
6.125232	399.949288	8.486784
6.429084	395.279017	8.491802
6.269312	401.744614	8.496819
6.446336	394.200365	8.501837
6.415711	394.202031	8.506854
6.637819	391.968021	8.511872
6.524649	381.269139	8.516890
5.818405	387.071929	8.521907
6.274003	390.115665	8.526925
6.242641	396.075298	8.531942
6.088109	403.382637	8.536960
6.494294	401.659581	8.541978
6.251143	400.589862	8.546995
6.299927	394.706513	8.552013
6.251759	401.385096	8.557030
6.303233	401.869416	8.562048
6.436647	395.467988	8.567066
6.480977	405.114252	8.572083
6.652495	399.397976	8.577101
6.256927	403.700804	8.582119
6.633652	395.538511	8.587136
6.328562	395.314681	8.592154
6.331568	408.366009	8.597171
6.107275	403.115281	8.602189
6.509925	403.122067	8.607207
6.152400	404.389554	8.612224
6.536275	400.082344	8.617242
6.232759	408.886567	8.622259
6.366403	402.235804	8.627277
6.462726	397.821894	8.632295
6.532213	391.970035	8.637312
6.474799	398.343959	8.642330
6.251606	405.630433	8.647347
6.632543	401.860139	8.652365
6.605887	401.611891	8.657383
6.263871	407.531539	8.662400
6.152407	399.401075	8.667418
6.075946	398.800839	8.672435
6.546806	399.516492	8.677453
6.265905	399.402499	8.682471
6.087516	400.383332	8.687488
6.696597	405.747818	8.692506
6.369620	410.210372	8.697523
6.535866	403.504043	8.702541
6.504715	420.363249	8.707559
6.497096	420.916727	8.712576
7.034871	412.972336	8.717594
6.909517	406.134691	8.722611
6.337448	398.189546	8.727629
6.688082	402.694912	8.732647
6.537621	396.306125	8.737664
6.611143	392.422759	8.742682
6.308473	397.825063	8.747699
6.375414	393.008651	8.752717
6.362621	400.704154	8.757735
6.299216	409.663487	8.762752
6.566479	417.507887	8.767770
6.637880	424.063725	8.772787
6.996989	424.433879	8.777805
6.922945	425.407934	8.782823
6.727896	413.143958	8.787840
6.983398	405.852559	8.792858
6.649367	403.916564	8.797875
6.832529	395.844366	8.802893
6.775883	406.449890	8.807911
6.350240	396.143616	8.812928
6.658247	391.706216	8.817946
6.695745	400.066040	8.822963
6.575038	397.178540	8.827981
6.770747	396.693710	8.832999
6.220137	395.599282	8.838016
6.439575	397.849856	8.843034
6.583736	409.683218	8.848051
6.507669	418.120690	8.853069
7.160868	420.477291	8.858087
6.774089	414.462946	8.863104
6.832230	396.059698	8.868122
6.659532	398.046295	8.873139
6.325362	401.515940	8.878157
6.737050	410.789447	8.883175
6.971513	424.855579	8.888192
7.084831	414.645251	8.893210
6.708395	404.391267	8.898227
6.518208	402.054200	8.903245
6.555624	414.636295	8.908263
6.915526	410.430640	8.913280
7.193314	419.870159	8.918298
6.768563	397.524956	8.923315
6.949457	392.280568	8.928333
6.912775	398.629175	8.933351
6.501932	405.499920	8.938368
6.649621	402.160397	8.943386
6.996846	414.978264	8.948403
6.879946	408.748341	8.953421
7.173493	397.563268	8.958439
6.512845	403.374742	8.963456
6.693865	402.150623	8.968474
6.585414	403.373018	8.973491
6.870794	415.569386	8.978509
7.117340	409.529016	8.983527
6.721616	409.442367	8.988544
7.017178	421.353146	8.993562
6.968057	416.267634	8.998579
6.638754	406.798378	9.003597
7.002526	417.493077	9.008615
6.912473	422.291113	9.013632
6.940543	412.125615	9.018650
6.851827	408.482090	9.023667
6.979873	417.301170	9.028685
6.958962	413.252631	9.033703
6.844390	414.756832	9.038720
7.192749	415.056080	9.043738
6.928055	405.807127	9.048755
6.781348	404.510964	9.053773
6.890019	412.777665	9.058791
6.875906	417.134708	9.063808
7.007667	425.145369	9.068826
7.131335	429.051794	9.073843
7.029704	419.196806	9.078861
6.977802	405.149697	9.083879
6.774167	405.784184	9.088896
6.910139	419.685776	9.093914
6.920568	420.665612	9.098931
7.276750	424.116134	9.103949
7.106962	426.903815	9.108967
7.004580	422.609195	9.113984
6.919170	414.275862	9.119002
6.854483	421.310456	9.124019
6.891205	427.805427	9.129037
7.336257	423.110008	9.134055
7.077741	426.069286	9.139072
7.341641	419.070050	9.144090
6.933652	411.471718	9.149107
6.582748	422.350273	9.154125
7.260736	416.567758	9.159143
6.912300	420.159542	9.164160
7.029786	424.467696	9.169178
6.780699	422.666790	9.174195
6.922762	431.218621	9.179213
7.131595	422.214653	9.184231
6.741794	425.020811	9.189248
7.176005	429.405879	9.194266
7.191190	428.138154	9.199283
7.102513	425.696920	9.204301
7.042593	421.061191	9.209319
6.959180	418.344597	9.214336
6.960439	419.938057	9.219354
7.099225	427.783531	9.224371
6.947904	432.938230	9.229389
7.178266	424.451591	9.234407
6.963252	432.465757	9.239424
7.226820	419.294123	9.244442
7.034300	424.613017	9.249459
6.775889	430.993002	9.254477
7.394442	440.486768	9.259495
7.046223	451.547951	9.264512
7.232716	450.272486	9.269530
7.350329	451.122032	9.274547
7.420804	458.460629	9.279565
7.423234	450.236673	9.284583
7.189232	438.341644	9.289600
7.270140	449.591619	9.294618
7.367712	437.553452	9.299635
6.854316	445.756084	9.304653
7.202608	443.414063	9.309671
7.058076	448.018626	9.314688
7.046077	450.497735	9.319706
7.012343	454.365560	9.324723
6.934752	463.715274	9.329741
7.142986	444.162039	9.334759
7.115858	459.168288	9.339776
6.994968	456.006265	9.344794
7.066714	449.267297	9.349811
6.916813	459.272020	9.354829
7.730175	461.701516	9.359847
7.308720	464.802929	9.364864
7.083627	455.595119	9.369882
7.389438	463.029614	9.374899
7.482844	476.196298	9.379917
7.960281	466.541445	9.384935
7.461795	458.805712	9.389952
7.621050	453.908642	9.394970
7.445450	446.532876	9.399987
7.199157	451.957976	9.405005
7.532530	452.966423	9.410023
7.506710	455.318303	9.415040
7.167627	453.446203	9.420058
7.272374	449.270799	9.425075
7.228180	457.826397	9.430093
7.546749	446.151427	9.435111
7.305200	450.632247	9.440128
7.212510	455.790447	9.445146
7.302054	457.243937	9.450163
7.261637	469.566804	9.455181
7.529258	467.726466	9.460199
7.441315	481.760795	9.465216
7.797779	474.822860	9.470234
7.445917	475.010235	9.475251
7.032953	479.072804	9.480269
7.359982	471.836510	9.485287
7.420915	477.967985	9.490304
7.528367	480.557882	9.495322
7.655829	473.459952	9.500339
7.327936	479.109193	9.505357
7.715423	469.506211	9.510375
7.682979	482.755608	9.515392
7.882788	483.257859	9.520410
7.962927	472.976927	9.525427
7.564484	468.501184	9.530445
7.442583	467.358937	9.535463
7.314436	460.341833	9.540480
7.640926	482.806659	9.545498
7.510534	468.531890	9.550515
7.787190	488.779745	9.555533
7.899546	477.076904	9.560551
7.861908	473.374922	9.565568
7.536812	453.352474	9.570586
7.385776	450.674805	9.575603
7.089206	457.758140	9.580621
7.734372	467.427650	9.585639
7.910125	474.390117	9.590656
7.749504	476.570493	9.595674
7.538812	460.989168	9.600691
7.564560	465.507266	9.605709
7.817604	477.232207	9.610727
7.585239	485.343767	9.615744
7.666740	483.232619	9.620762
7.811537	474.143925	9.625779
7.713578	474.247590	9.630797
7.646690	471.159203	9.635815
7.626681	479.830961	9.640832
7.822572	483.470546	9.645850
7.899321	477.835269	9.650867
7.789682	477.372733	9.655885
7.745523	474.110402	9.660903
7.790822	473.917219	9.665920
7.605323	461.989377	9.670938
7.538650	466.802718	9.675955
7.748680	473.135029	9.680973
8.065821	476.064644	9.685991
7.913781	464.074790	9.691008
7.636597	469.763467	9.696026
7.579921	471.031452	9.701043
7.965595	476.588526	9.706061
7.825953	474.830532	9.711079
7.677140	472.619551	9.716096
7.617644	475.680388	9.721114
7.718612	471.802198	9.726131
7.977854	493.984032	9.731149
7.828973	489.986956	9.736167
7.490117	478.259697	9.741184
7.657420	481.831152	9.746202
7.981535	482.774774	9.751219
7.987171	480.953136	9.756237
8.083630	482.676939	9.761255
7.925865	473.591175	9.766272
7.854993	485.306596	9.771290
7.708248	486.648563	9.776307
8.090637	481.902928	9.781325
7.873902	485.240701	9.786343
7.875886	484.101253	9.791360
7.643702	487.580281	9.796378
7.788387	475.083493	9.801395
8.004327	479.849681	9.806413
7.777595	483.529821	9.811431
7.664062	482.313689	9.816448
7.469804	484.272096	9.821466
7.817384	479.724376	9.826483
7.721155	489.610311	9.831501
7.733068	494.244174	9.836519
8.375738	509.124090	9.841536
7.970992	499.950540	9.846554
7.933799	489.164028	9.851571
7.838541	506.932660	9.856589
8.016948	506.665106	9.861607
8.245451	514.925820	9.866624
8.149649	509.219573	9.871642
8.301240	495.087063	9.876659
8.200020	489.962307	9.881677
7.992416	481.446006	9.886695
8.129409	480.490656	9.891712
7.837693	482.776646	9.896730
7.901640	487.793708	9.901747
7.864169	494.435947	9.906765
7.852219	499.379626	9.911783
8.181284	506.870476	9.916800
7.695067	512.402374	9.921818
7.947551	510.722172	9.926835
8.163295	513.957902	9.931853
8.347222	507.349762	9.936871
8.491972	504.764882	9.941888
8.302696	504.232697	9.946906
7.963170	504.740030	9.951923
7.988160	507.569978	9.956941
7.840326	501.477376	9.961959
8.213001	505.266157	9.966976
8.231001	514.815600	9.971994
8.065607	506.037106	9.977011
8.337832	499.263750	9.982029
7.743574	500.659616	9.987047
8.145993	502.629260	9.992064
7.796514	505.100964	9.997082
7.759493	500.591030	10.002099
7.953475	514.029248	10.007117
8.293786	524.020797	10.012135
8.485297	529.586028	10.017152
8.303810	522.447823	10.022170
8.235745	514.663983	10.027187
8.515538	521.805922	10.032205
8.411594	520.635630	10.037223
8.063398	510.071088	10.042240
8.115472	514.484119	10.047258
8.287644	524.123166	10.052275
8.364830	529.362230	10.057293
8.321970	523.928590	10.062311
8.690266	522.593257	10.067328
8.002382	518.358218	10.072346
8.312845	517.558885	10.077363
8.449271	527.989261	10.082381
8.235850	523.844442	10.087399
8.610761	530.211059	10.092416
8.440038	522.477913	10.097434
8.114303	518.255913	10.102451
8.080380	523.143062	10.107469
8.338797	531.597933	10.112487
8.701721	529.685949	10.117504
8.585318	531.218847	10.122522
8.236200	535.101081	10.127539
8.788892	532.575752	10.132557
8.106238	520.444422	10.137575
8.378544	532.305249	10.142592
8.396536	533.328094	10.147610
8.658538	537.389722	10.152627
8.719973	538.244864	10.157645
8.610428	532.897339	10.162663
8.467499	522.546973	10.167680
8.341364	523.466031	10.172698
8.318823	518.404752	10.177715
8.703069	533.656270	10.182733
8.400307	528.341985	10.187751
8.608336	519.454854	10.192768
8.764805	532.520246	10.197786
8.617404	520.434961	10.202803
8.360242	503.806842	10.207821
8.131702	506.404877	10.212839
8.596043	521.022247	10.217856
8.674142	525.289223	10.222874
8.656586	527.772364	10.227891
9.190911	526.739369	10.232909
8.689619	514.784924	10.237927
8.786045	506.107670	10.242944
8.190656	505.490401	10.247962
8.695470	497.260784	10.252979
8.592340	502.149235	10.257997
8.303472	505.788564	10.263015
8.537149	506.266608	10.268032
8.448989	522.440541	10.273050
9.057934	524.674664	10.278067
8.901866	522.019858	10.283085
8.939269	514.976957	10.288103
8.804826	506.237824	10.293120
8.931338	511.081056	10.298138
8.529829	500.341793	10.303155
8.423499	501.166251	10.308173
8.563377	498.285498	10.313191
8.594554	493.869085	10.318208
8.392429	501.947543	10.323226
8.965632	514.149656	10.328243
8.737444	512.837770	10.333261
8.930486	521.536335	10.338279
8.827216	508.762563	10.343296
8.584484	507.276225	10.348314
8.470339	512.623965	10.353331
8.590641	520.699566	10.358349
9.029521	523.657571	10.363367
8.780430	531.257383	10.368384
8.973181	525.799680	10.373402
9.174099	521.094912	10.378419
8.604337	509.804353	10.383437
8.428421	522.495475	10.388455
8.853075	523.574918	10.393472
8.776954	527.417802	10.398490
9.045319	524.523351	10.403507
8.929707	526.182351	10.408525
9.136411	529.984356	10.413543
9.072347	518.258466	10.418560
8.697619	506.502061	10.423578
8.404427	510.243045	10.428595
8.972218	516.822612	10.433613
9.022476	526.789897	10.438631
8.796109	519.699704	10.443648
9.214574	530.594231	10.448666
8.759560	519.639234	10.453683
9.042470	512.857897	10.458701
8.544539	525.794810	10.463719
9.220894	521.795467	10.468736
9.114360	527.725825	10.473754
9.160558	526.803543	10.478771
9.107999	521.970989	10.483789
8.887304	522.759609	10.488807
8.713777	526.829088	10.493824
9.208221	525.884350	10.498842
8.820777	535.503242	10.503859
8.850345	528.537291	10.508877
8.888014	541.681146	10.513895
9.050835	535.634835	10.518912
9.000750	532.477553	10.523930
8.817025	535.153817	10.528947
9.112353	525.965924	10.533965
9.001413	537.290004	10.538983
8.897311	524.472171	10.544000
8.641470	528.270456	10.549018
8.826286	528.857090	10.554035
8.958194	524.188311	10.559053
8.644091	528.525819	10.564071
9.169566	538.785179	10.569088
8.945310	538.365732	10.574106
9.129041	549.880616	10.579123
9.465720	555.391697	10.584141
9.137490	556.796638	10.589159
9.303092	557.364175	10.594176
9.071396	543.843545	10.599194
8.992842	545.932260	10.604211
9.319007	551.751076	10.609229
9.002554	555.022341	10.614247
9.286760	548.426974	10.619264
9.549446	546.852473	10.624282
8.986582	545.898792	10.629299
9.313174	541.467929	10.634317
9.288041	549.919622	10.639335
9.290839	555.271257	10.644352
9.173967	559.448682	10.649370
9.616539	563.781991	10.654387
9.436348	545.292625	10.659405
9.064069	547.647969	10.664423
9.077517	530.630568	10.669440
9.375491	535.374531	10.674458
8.993243	542.717381	10.679475
9.398422	547.290027	10.684493
9.311661	551.907712	10.689511
9.046634	548.446236	10.694528
9.274714	547.943740	10.699546
9.306102	558.485157	10.704563
9.639998	556.533511	10.709581
9.584645	561.133685	10.714599
9.635844	557.471500	10.719616
10.023502	544.756960	10.724634
9.296619	538.839705	10.729651
9.225935	535.654073	10.734669
8.890027	530.843544	10.739687
9.251337	551.169804	10.744704
9.587711	559.000351	10.749722
9.673261	555.629451	10.754739
9.395768	556.164995	10.759757
9.495602	556.477695	10.764775
9.686213	553.592189	10.769792
9.477015	535.018991	10.774810
9.507472	540.158041	10.779827
9.411234	535.108233	10.784845
9.492157	544.408064	10.789863
9.355169	544.603008	10.794880
9.558675	553.946871	10.799898
9.419677	557.521852	10.804915
9.814626	553.720944	10.809933
9.563610	550.430848	10.814951
9.257245	558.942111	10.819968
9.454027	559.520571	10.824986
9.137332	558.361312	10.830003
9.336663	556.405371	10.835021
9.329011	555.100169	10.840039
9.385358	561.434349	10.845056
9.455151	559.031537	10.850074
9.376960	563.382814	10.855091
9.325713	551.654906	10.860109
9.206843	554.062310	10.865127
9.514390	562.941874	10.870144
9.950556	577.954982	10.875162
9.602184	578.416358	10.880179
9.188409	577.897036	10.885197
9.398723	576.188681	10.890215
9.502352	580.233954	10.895232
10.021633	586.650694	10.900250
9.831521	592.701379	10.905267
10.237700	586.093319	10.910285
10.206450	577.517957	10.915303
9.555849	578.165239	10.920320
9.741711	562.992278	10.925338
9.325884	566.361064	10.930355
9.607799	576.737259	10.935373
9.586726	576.431338	10.940391
9.616635	579.677080	10.945408
10.031627	578.511190	10.950426
10.032199	571.865305	10.955443
10.129034	577.751393	10.960461
10.038015	577.213375	10.965479
9.381909	568.580678	10.970496
9.846674	565.911251	10.975514
9.609018	571.997732	10.980531
9.933011	580.455040	10.985549
9.601704	581.604853	10.990567
9.699896	578.793690	10.995584
9.971242	577.202060	11.000602
9.722501	580.039926	11.005619
9.891147	576.870670	11.010637
10.067041	585.477266	11.015655
9.653723	582.332350	11.020672
10.022551	581.006397	11.025690
9.893436	583.396466	11.030707
10.226797	583.799034	11.035725
10.198016	583.099853	11.040743
9.979473	592.613586	11.045760
9.998937	593.039782	11.050778
10.231877	591.151185	11.055795
10.271472	585.064085	11.060813
9.779657	576.790797	11.065831
10.137868	585.593059	11.070848
10.108299	577.285668	11.075866
9.763464	576.654630	11.080883
10.214212	580.873066	11.085901
10.218553	580.361225	11.090919
9.838828	573.683036	11.095936
9.942625	579.527016	11.100954
10.221183	593.842027	11.105971
10.139547	595.685084	11.110989
10.236817	583.612153	11.116007
9.809033	583.552584	11.121024
10.084737	583.285659	11.126042
10.170713	588.460258	11.131059
9.819085	588.171091	11.136077
10.052755	577.345508	11.141095
9.944397	590.127142	11.146112
10.057877	591.343397	11.151130
9.914852	593.786124	11.156147
10.038713	589.194317	11.161165
9.873791	582.672021	11.166183
10.011235	587.437836	11.171200
10.276609	580.488798	11.176218
9.932827	587.790965	11.181235
10.095428	586.030080	11.186253
9.949165	578.715961	11.191271
9.929691	580.123323	11.196288
10.193874	595.848004	11.201306
10.330202	609.254247	11.206323
10.486584	608.185423	11.211341
10.367638	611.810939	11.216359
10.078155	606.207397	11.221376
10.213995	608.414211	11.226394
10.475783	613.551977	11.231411
10.497000	610.686525	11.236429
10.534687	597.521529	11.241447
10.002281	596.096062	11.246464
10.482583	600.161585	11.251482
10.336929	605.940276	11.256499
10.062744	596.440246	11.261517
10.279862	595.437703	11.266535
10.394000	611.570752	11.271552
10.525837	609.824122	11.276570
10.562640	605.050214	11.281587
10.324427	605.626978	11.286605
10.540529	615.843036	11.291623
10.391175	612.786399	11.296640
10.466589	618.151993	11.301658
10.762784	608.515815	11.306675
10.537148	605.086064	11.311693
10.375093	596.247047	11.316711
10.419609	602.747180	11.321728
10.500861	605.407443	11.326746
10.593914	609.457525	11.331763
10.572335	596.279667	11.336781
10.465834	598.937605	11.341799
10.664337	606.328910	11.346816
10.644134	596.379099	11.351834
10.150073	592.382097	11.356851
10.291280	600.303007	11.361869
10.627871	599.799392	11.366887
10.742436	597.351737	11.371904
10.576983	601.502023	11.376922
10.924239	604.875078	11.381939
10.898231	603.115156	11.386957
10.853210	587.905541	11.391975
10.359661	590.787836	11.396992
10.323719	588.177430	11.402010
10.251180	600.448586	11.407027
10.646470	600.027347	11.412045
11.043043	598.110117	11.417063
10.694114	607.372770	11.422080
10.639476	601.786311	11.427098
10.855170	607.262598	11.432115
10.699656	612.894510	11.437133
10.857266	591.641771	11.442151
10.767597	592.249054	11.447168
10.510002	590.578837	11.452186
10.821493	604.178701	11.457203
10.708705	605.739443	11.462221
10.938342	603.409565	11.467239
10.739585	595.990007	11.472256
10.841021	600.789833	11.477274
10.771076	588.222246	11.482291
10.584005	595.878698	11.487309
10.508729	591.197980	11.492327
10.753948	608.967349	11.497344
11.091249	604.695742	11.502362
11.011764	608.217288	11.507379
10.832137	615.509686	11.512397
11.153513	603.146238	11.517415
10.732350	596.676456	11.522432
11.128672	602.736820	11.527450
10.902193	585.400131	11.532467
10.706147	582.596912	11.537485
10.455247	582.702299	11.542503
10.570411	604.903548	11.547520
10.808199	607.416369	11.552538
10.405368	615.762804	11.557555
10.578704	606.417145	11.562573
10.797981	603.233690	11.567591
10.767772	603.042796	11.572608
10.772891	600.545911	11.577626
10.813290	612.076840	11.582643
11.040332	626.898496	11.587661
11.232061	622.848358	11.592679
11.147985	623.801895	11.597696
11.086027	614.057383	11.602714
10.926024	606.666500	11.607731
10.915956	611.262792	11.612749
11.172360	621.188567	11.617767
10.701535	620.485629	11.622784
10.866642	631.656341	11.627802
11.290075	626.216338	11.632819
10.919511	628.552491	11.637837
11.320995	630.699014	11.642855
11.139681	640.509921	11.647872
11.301787	625.432121	11.652890
11.508801	625.415722	11.657907
11.639323	631.425965	11.662925
11.290977	609.188516	11.667943
11.025464	601.779350	11.672960
11.140838	598.997066	11.677978
10.961360	602.786633	11.682995
11.068244	616.983231	11.688013
11.107400	621.174245	11.693031
11.169768	626.147412	11.698048
11.412878	633.610675	11.703066
11.311756	633.841060	11.708083
11.374061	634.667670	11.713101
11.683536	633.505583	11.718119
11.039884	620.459274	11.723136
11.063086	620.673458	11.728154
11.164304	627.830620	11.733171
11.418345	632.016581	11.738189
11.090092	636.880163	11.743207
11.303897	637.806256	11.748224
11.261952	631.394178	11.753242
11.407779	623.027900	11.758259
10.970613	632.970153	11.763277
11.725844	629.302475	11.768295
11.262977	625.284831	11.773312
11.217061	631.941059	11.778330
11.498190	628.943622	11.783347
11.145281	635.912727	11.788365
11.329148	632.633799	11.793383
11.467345	640.596219	11.798400
10.939245	638.882912	11.803418
10.979190	634.234733	11.808435
11.206146	634.275187	11.813453
11.564460	640.739099	11.818471
11.857668	652.887076	11.823488
11.596341	650.775638	11.828506
11.339084	634.756459	11.833523
11.369556	642.218121	11.838541
11.431561	641.507958	11.843559
11.370777	650.776262	11.848576
11.725505	653.731612	11.853594
12.026572	652.725461	11.858611
11.591410	647.977689	11.863629
11.877358	632.350446	11.868647
11.918846	633.372793	11.873664
11.493716	629.494433	11.878682
11.701618	635.391649	11.883699
11.113794	638.850341	11.888717
11.148732	628.835124	11.893735
11.300454	642.213749	11.898752
11.405091	654.283793	11.903770
11.690142	657.966334	11.908787
11.540082	658.671381	11.913805
12.207215	652.631714	11.918823
12.268261	665.588990	11.923840
11.927739	667.645926	11.928858
11.908950	647.389383	11.933875
11.447720	642.872880	11.938893
11.985437	649.596030	11.943911
11.687929	642.949193	11.948928
11.470728	652.765695	11.953946
11.883038	653.979607	11.958963
11.653760	663.384600	11.963981
11.813196	661.763051	11.968999
12.264416	661.844325	11.974016
12.222105	655.738397	11.979034
11.713570	644.154207	11.984051
11.407133	641.696357	11.989069
11.843677	648.056576	11.994087
11.759420	646.384612	11.999104
11.795627	654.978277	12.004122
12.062841	651.402356	12.009139
11.588446	654.417373	12.014157
11.638637	650.209392	12.019175
11.728411	643.303448	12.024192
11.546051	658.838945	12.029210
11.925760	659.038646	12.034227
11.908907	662.039228	12.039245
12.055872	648.835090	12.044263
11.940644	657.196723	12.049280
11.878303	656.761532	12.054298
12.268418	649.395428	12.059315
11.765445	660.651242	12.064333
12.144107	658.462249	12.069351
12.441836	654.307241	12.074368
12.258267	655.168978	12.079386
12.346836	657.723972	12.084403
12.247207	656.461484	12.089421
11.841407	659.418487	12.094439
11.781946	655.786134	12.099456
11.931574	663.955061	12.104474
11.862061	653.085122	12.109491
11.779153	659.393683	12.114509
11.798136	668.046839	12.119527
11.726155	672.791637	12.124544
11.995049	676.536655	12.129562
12.162852	673.989185	12.134579
12.309331	686.961576	12.139597
11.904659	686.166287	12.144615
12.430666	681.496065	12.149632
12.494905	693.834349	12.154650
12.289178	681.552915	12.159667
12.445240	685.400707	12.164685
12.182508	679.474251	12.169703
12.466462	684.286706	12.174720
11.778666	696.297128	12.179738
12.552707	692.181556	12.184755
12.276232	684.051408	12.189773
12.071226	676.310909	12.194791
12.667598	683.422557	12.199808
12.019829	687.575377	12.204826
12.148075	677.633964	12.209843
12.201520	684.432527	12.214861
11.943061	680.001205	12.219879
12.471078	682.203770	12.224896
12.187626	689.521831	12.229914
12.227672	683.390448	12.234931
12.326805	680.194128	12.239949
12.471541	688.537391	12.244967
12.390185	681.702257	12.249984
12.339771	685.607441	12.255002
12.526336	680.778638	12.260019
12.787913	699.801517	12.265037
12.683545	694.986450	12.270055
12.519218	690.474200	12.275072
12.451472	686.537028	12.280090
12.407351	685.972771	12.285107
12.483000	679.337246	12.290125
12.468150	681.106800	12.295143
12.556096	688.966617	12.300160
12.790259	691.259115	12.305178
12.768123	687.523118	12.310195
12.774608	676.742314	12.315213
12.599638	684.756669	12.320231
12.821233	681.427678	12.325248
12.926453	683.146981	12.330266
12.810346	678.314812	12.335283
12.442303	678.807655	12.340301
12.480923	679.798895	12.345319
12.785459	680.613037	12.350336
12.417996	682.080899	12.355354
12.351392	688.462669	12.360371
12.386214	687.223425	12.365389
12.966913	703.255514	12.370407
13.273883	700.272976	12.375424
12.898961	686.111841	12.380442
12.777494	680.037164	12.385459
12.524457	682.490720	12.390477
12.692446	690.678890	12.395495
13.166608	682.472895	12.400512
13.145554	689.601784	12.405530
12.586736	685.021572	12.410547
12.940054	685.676647	12.415565
12.784641	680.209992	12.420583
12.835521	680.176878	12.425600
12.777656	681.255722	12.430618
12.763232	678.329539	12.435635
13.058586	685.548013	12.440653
12.907184	683.167001	12.445671
12.711293	686.457386	12.450688
12.635774	699.988196	12.455706
12.735673	694.835223	12.460723
12.925648	702.414082	12.465741
12.604586	711.259054	12.470759
13.059846	715.224364	12.475776
12.633793	714.467115	12.480794
12.873312	710.747177	12.485811
12.866526	711.770734	12.490829
12.817074	719.090242	12.495847
13.115336	709.172831	12.500864
12.458708	713.951865	12.505882
12.778918	713.750590	12.510899
12.761861	726.770562	12.515917
12.911633	726.109845	12.520935
13.145680	732.479533	12.525952
13.129923	737.559566	12.530970
13.196212	734.904820	12.535987
13.654202	732.987481	12.541005
12.897604	731.789407	12.546023
13.453552	720.642169	12.551040
13.170376	729.970385	12.556058
13.454688	734.495629	12.561075
13.529947	731.631210	12.566093
12.867666	726.139321	12.571111
13.383975	727.412783	12.576128
13.303357	737.469989	12.581146
13.439877	731.699097	12.586163
13.402749	713.304043	12.591181
13.034495	718.915463	12.596199
13.470420	708.793589	12.601216
13.360949	713.544235	12.606234
13.232450	712.349352	12.611251
13.684157	707.188935	12.616269
13.272877	711.913990	12.621287
13.303175	696.654687	12.626304
12.968113	707.654021	12.631322
13.236665	717.426485	12.636339
13.575852	725.411297	12.641357
13.568002	743.513683	12.646375
13.673259	732.345094	12.651392
13.493396	731.132961	12.656410
13.210435	726.787490	12.661427
13.414051	731.221159	12.666445
13.091368	737.753267	12.671463
13.800450	733.054527	12.676480
13.652731	731.209405	12.681498
13.819938	736.264106	12.686515
13.670870	730.922676	12.691533
13.043182	715.838384	12.696551
13.364365	716.044042	12.701568
13.555186	731.543589	12.706586
13.414433	735.630102	12.711603
13.425706	732.788268	12.716621
13.189818	732.127639	12.721639
13.807818	735.935077	12.726656
13.474089	742.768698	12.731674
13.181333	736.225224	12.736691
13.374027	738.366400	12.741709
13.377025	739.899659	12.746727
13.765993	735.900834	12.751744
13.684546	734.158999	12.756762
13.456052	737.078941	12.761779
13.899138	745.959584	12.766797
13.358121	760.882001	12.771815
13.898174	761.662634	12.776832
13.879814	756.143060	12.781850
13.647728	760.691909	12.786867
13.718381	766.825126	12.791885
13.785190	762.702891	12.796903
13.892187	762.793580	12.801920
13.867627	764.331131	12.806938
13.801536	768.617460	12.811955
13.690313	757.220637	12.816973
13.682835	760.267112	12.821991
13.751746	760.912824	12.827008
13.684053	756.227726	12.832026
13.416513	762.479866	12.837043
13.752798	760.250124	12.842061
13.896389	765.116012	12.847079
13.916935	762.739775	12.852096
13.586714	763.412918	12.857114
13.564367	755.612388	12.862131
14.034728	769.537926	12.867149
13.849784	779.128575	12.872167
14.133989	778.958151	12.877184
14.436433	773.710506	12.882202
13.927249	770.249132	12.887219
14.104999	764.897831	12.892237
13.903289	767.864099	12.897255
14.100521	766.482802	12.902272
13.926210	777.450839	12.907290
14.324294	772.096787	12.912307
14.128604	763.449112	12.917325
13.897887	766.113792	12.922343
14.081660	773.709426	12.927360
14.290166	779.044878	12.932378
14.268216	779.849900	12.937395
14.580495	770.738135	12.942413
14.133455	763.035283	12.947431
14.037859	763.103868	12.952448
14.023548	767.000293	12.957466
14.167431	776.410360	12.962483
14.260653	769.873048	12.967501
14.275489	772.294377	12.972519
14.494651	773.194398	12.977536
14.235182	783.591891	12.982554
14.141883	783.552825	12.987571
14.589332	773.242932	12.992589
14.073431	775.311407	12.997607
14.206741	775.962872	13.002624
14.251687	774.343360	13.007642
14.143016	780.697000	13.012659
14.164338	778.689858	13.017677
14.124146	786.074222	13.022695
14.528467	778.500732	13.027712
14.643490	778.558614	13.032730
14.307157	780.987285	13.037747
14.469523	778.636300	13.042765
14.313236	781.109519	13.047783
14.403131	778.877112	13.052800
14.592662	776.667061	13.057818
14.488372	776.607615	13.062835
14.816964	774.173948	13.067853
14.696738	778.645427	13.072871
14.369066	769.945716	13.077888
14.689500	774.216045	13.082906
14.379310	770.496478	13.087923
14.700514	771.519463	13.092941
14.623539	769.590741	13.097959
14.551777	760.866968	13.102976
15.006719	766.971909	13.107994
15.055352	782.114953	13.113011
14.362395	771.108488	13.118029
14.541401	781.829019	13.123047
14.620178	779.831865	13.128064
14.669204	772.828077	13.133082
14.334202	777.721149	13.138099
14.300205	773.996447	13.143117
14.351956	784.399132	13.148135
14.736114	793.655036	13.153152
14.795851	798.338335	13.158170
14.605253	803.215242	13.163187
14.987065	800.290460	13.168205
14.663862	803.158889	13.173223
14.358420	809.808255	13.178240
14.542068	806.333675	13.183258
14.720183	812.642674	13.188275
14.589157	806.673580	13.193293
14.823369	810.796401	13.198311
14.722973	803.588653	13.203328
14.726362	803.272608	13.208346
14.614313	805.060464	13.213363
14.576607	799.354546	13.218381
14.870628	819.284502	13.223399
15.254169	823.156864	13.228416
15.385876	826.588768	13.233434
15.040898	819.816715	13.238451
14.834180	809.513983	13.243469
15.186884	805.637550	13.248487
14.631559	811.360175	13.253504
15.387809	812.305959	13.258522
15.014927	807.939756	13.263539
15.612067	813.107416	13.268557
15.311325	813.984248	13.273575
15.080226	808.226389	13.278592
15.164317	808.418471	13.283610
15.004317	809.345972	13.288627
15.299594	799.208076	13.293645
15.024096	796.593913	13.298663
14.928539	803.204287	13.303680
15.226283	798.815721	13.308698
15.174544	799.814724	13.313715
15.427862	799.049523	13.318733
15.555463	790.613423	13.323751
15.447195	802.142377	13.328768
15.431241	797.575441	13.333786
15.369505	800.412627	13.338803
15.415587	790.966767	13.343821
15.462542	802.417906	13.348839
15.211775	800.109152	13.353856
15.622606	791.909812	13.358874
15.102491	797.273510	13.363891
15.293229	797.777183	13.368909
15.352681	797.903676	13.373927
15.061066	798.043805	13.378944
15.503403	797.107167	13.383962
15.518903	799.269627	13.388979
15.168820	798.008255	13.393997
15.660098	795.953186	13.399015
15.380425	799.124097	13.404032
15.417542	795.217910	13.409050
15.644065	793.573281	13.414067
15.320690	798.278361	13.419085
16.015556	792.764490	13.424103
15.420624	804.858353	13.429120
15.473608	796.134075	13.434138
15.250112	799.946315	13.439155
15.426517	815.445024	13.444173
15.636439	804.282184	13.449191
15.179857	816.083122	13.454208
15.408211	819.105512	13.459226
15.749226	822.375442	13.464243
15.558817	818.116522	13.469261
15.951543	819.213578	13.474279
15.802873	819.479769	13.479296
15.883856	822.682891	13.484314
15.801502	821.045327	13.489331
15.718925	825.621406	13.494349
15.996173	823.135768	13.499367
15.808072	817.248138	13.504384
16.126252	821.758664	13.509402
15.930277	834.825506	13.514419
15.705883	823.345278	13.519437
15.948990	825.273494	13.524455
15.783150	824.422079	13.529472
16.018988	820.595396	13.534490
15.570191	824.300714	13.539507
16.057750	820.075087	13.544525
15.983674	816.618541	13.549543
15.891750	820.662758	13.554560
16.185519	821.450183	13.559578
16.019560	818.484456	13.564595
15.677785	805.731827	13.569613
15.603179	812.095952	13.574631
15.572179	820.532909	13.579648
16.055801	823.752234	13.584666
16.112891	830.739628	13.589683
15.782546	829.945383	13.594701
15.975640	825.311179	13.599719
15.962092	833.448786	13.604736
15.884993	822.794514	13.609754
16.055618	821.231167	13.614771
15.723295	830.800611	13.619789
15.841775	833.344662	13.624807
15.775998	829.097892	13.629824
16.239493	840.105515	13.634842
16.226860	846.412668	13.639859
16.421379	838.502599	13.644877
16.159167	845.410328	13.649895
16.362238	846.454866	13.654912
16.679188	837.194021	13.659930
16.378994	830.777899	13.664947
16.105657	830.457603	13.669965
16.186027	823.780266	13.674983
15.975351	840.188151	13.680000
16.428896	837.346866	13.685018
16.361301	844.852283	13.690035
16.181555	844.044057	13.695053
16.334012	840.366048	13.700071
16.156828	848.958318	13.705088
16.630454	851.027366	13.710106
16.345417	849.541274	13.715123
16.525910	840.633024	13.720141
16.830694	847.799604	13.725159
16.531008	851.260810	13.730176
16.256950	849.179733	13.735194
16.193070	854.169464	13.740211
15.802135	846.603003	13.745229
16.424650	840.756408	13.750247
16.215502	843.212620	13.755264
16.431174	850.882213	13.760282
16.525196	849.157226	13.765299
16.359617	845.645495	13.770317
16.693367	851.914498	13.775335
16.331341	864.066810	13.780352
16.908685	863.762384	13.785370
17.135120	873.405795	13.790387
16.509506	863.124072	13.795405
16.679005	853.987159	13.800423
16.312865	856.638224	13.805440
16.941476	863.167428	13.810458
16.902118	872.514559	13.815475
16.688478	867.934204	13.820493
16.787285	867.104696	13.825511
17.170767	870.459539	13.830528
16.596670	859.248325	13.835546
16.735342	856.654873	13.840563
16.695252	870.028821	13.845581
17.149859	858.872031	13.850599
16.859122	868.570715	13.855616
16.960885	848.159478	13.860634
16.696397	857.696284	13.865651
16.791199	865.517243	13.870669
16.839194	875.529256	13.875687
16.952321	884.508678	13.880704
17.026534	878.826333	13.885722
17.053923	881.987318	13.890739
16.994559	879.440475	13.895757
17.295887	868.743034	13.900775
17.231339	872.290707	13.905792
16.815211	865.122626	13.910810
16.796193	860.275292	13.915827
17.066967	878.217671	13.920845
17.123274	863.487494	13.925863
17.098730	876.316242	13.930880
16.874359	876.534262	13.935898
16.789366	880.173480	13.940915
17.056046	872.981134	13.945933
17.114117	874.161856	13.950951
17.136316	878.945692	13.955968
16.915893	878.746542	13.960986
17.169395	869.713303	13.966003
17.219256	881.334450	13.971021
17.170116	878.416795	13.976039
17.217963	883.171393	13.981056
16.990629	878.422758	13.986074
17.348690	874.305642	13.991091
17.144600	886.723706	13.996109
17.396751	874.411873	14.001127
17.242799	883.319271	14.006144
17.506820	897.466381	14.011162
17.452685	888.089721	14.016179
17.755784	878.124127	14.021197
17.850316	874.098533	14.026215
17.372956	876.820566	14.031232
17.328894	874.640561	14.036250
17.187666	875.401044	14.041267
17.231908	876.044290	14.046285
17.535731	889.408887	14.051303
17.649889	897.608689	14.056320
17.520936	903.511105	14.061338
17.556629	899.037085	14.066355
17.529629	903.746539	14.071373
17.908696	906.963224	14.076391
17.488229	895.226306	14.081408
17.385579	902.352206	14.086426
17.584630	905.884090	14.091443
17.247190	911.585445	14.096461
17.349231	897.880043	14.101479
17.508064	904.308839	14.106496
17.414639	909.858595	14.111514
17.581556	899.693292	14.116531
17.524084	902.545608	14.121549
17.547023	892.393259	14.126567
17.383372	913.647404	14.131584
17.870448	914.455228	14.136602
18.287585	921.209878	14.141619
17.916409	913.848590	14.146637
18.200667	900.553463	14.151655
17.996222	903.854687	14.156672
17.683305	904.083338	14.161690
17.662747	898.898569	14.166707
17.804110	902.672959	14.171725
17.968382	892.672169	14.176743
17.627511	903.309619	14.181760
18.055503	915.054946	14.186778
18.331937	912.282250	14.191795
17.953942	902.110270	14.196813
17.806796	897.831972	14.201831
18.187065	915.735251	14.206848
18.126254	914.798053	14.211866
17.919509	901.550971	14.216883
17.690305	906.307687	14.221901
18.191938	917.946879	14.226919
18.357336	922.569579	14.231936
18.337822	930.676603	14.236954
18.419708	919.902847	14.241971
17.909571	912.986063	14.246989
17.775500	914.597482	14.252007
17.681718	924.063564	14.257024
17.960063	930.284418	14.262042
18.115712	926.634296	14.267059
17.826064	934.155389	14.272077
18.151662	925.331799	14.277095
18.128711	936.468868	14.282112
18.267907	932.616184	14.287130
18.709098	927.577260	14.292147
18.632858	934.001642	14.297165
18.663995	928.815127	14.302183
18.540859	924.788699	14.307200
18.690007	929.871513	14.312218
18.733075	928.163919	14.317235
18.589114	932.891592	14.322253
18.402393	929.367357	14.327271
18.339463	924.122908	14.332288
18.315709	927.253995	14.337306
18.586632	931.017686	14.342323
18.755783	922.581366	14.347341
18.540709	927.913387	14.352359
18.838226	918.860648	14.357376
18.175236	926.714415	14.362394
18.647228	910.272184	14.367411
18.473805	925.863324	14.372429
18.472296	922.098820	14.377447
18.134959	911.781652	14.382464
17.972957	920.766059	14.387482
18.978512	922.758608	14.392499
18.692170	942.460334	14.397517
19.195452	935.641370	14.402535
19.160690	924.260937	14.407552
18.781270	936.160391	14.412570
18.707401	929.724775	14.417587
18.673741	918.063313	14.422605
18.777930	929.114311	14.427623
18.843741	932.332438	14.432640
18.694759	931.295360	14.437658
18.460044	923.149134	14.442675
19.079516	942.842368	14.447693
18.930246	947.936937	14.452711
19.215901	949.151656	14.457728
18.916499	936.872008	14.462746
18.550240	929.074456	14.467763
18.843949	942.162963	14.472781
18.954043	949.094814	14.477799
19.073363	956.798389	14.482816
18.951051	955.611994	14.487834
19.067784	942.642714	14.492851
18.984694	944.823698	14.497869
19.095085	948.170583	14.502887
19.243851	944.190177	14.507904
18.873974	951.531268	14.512922
19.319317	951.007557	14.517939
19.144708	954.657587	14.522957
19.061263	952.209155	14.527975
19.306476	954.206484	14.532992
19.297649	950.124383	14.538010
19.187190	950.009094	14.543027
18.992160	958.187638	14.548045
19.084973	957.172871	14.553063
19.570211	953.121141	14.558080
19.382914	960.358070	14.563098
19.438211	952.135119	14.568115
19.208539	953.979172	14.573133
19.288292	956.655500	14.578151
19.064512	956.116051	14.583168
19.142426	953.285897	14.588186
19.197625	950.172108	14.593203
19.241102	965.376069	14.598221
18.953512	959.803677	14.603239
19.236308	972.079724	14.608256
19.404683	978.866816	14.613274
19.407025	979.361957	14.618291
19.474137	975.277495	14.623309
19.264696	981.946691	14.628327
19.564404	975.777935	14.633344
19.631069	986.045874	14.638362
19.581503	981.203263	14.643379
19.448114	977.175263	14.648397
19.081851	981.558871	14.653415
19.709603	969.317879	14.658432
19.428935	987.709137	14.663450
19.263081	976.197606	14.668467
19.629786	997.097881	14.673485
19.377733	992.223679	14.678503
19.816742	996.469289	14.683520
20.081426	1000.751509	14.688538
20.048803	996.414331	14.693555
19.683744	1003.940883	14.698573
19.533527	1005.586381	14.703591
19.926636	999.952174	14.708608
19.770701	1008.121498	14.713626
19.994563	1002.409503	14.718643
19.958744	1007.454867	14.723661
19.485614	1010.037408	14.728679
20.016413	1001.803514	14.733696
19.975874	1000.266718	14.738714
19.728678	1000.204276	14.743731
19.983645	1000.852586	14.748749
19.953754	999.165812	14.753767
20.392674	996.115345	14.758784
20.003122	1004.564033	14.763802
20.117147	994.662527	14.768819
20.118423	997.931738	14.773837
19.861075	1005.567750	14.778855
20.275581	1002.641001	14.783872
20.131274	993.533941	14.788890
20.123499	993.330082	14.793907
20.189491	998.750905	14.798925
19.746957	998.027767	14.803943
20.092487	996.768527	14.808960
20.178578	1021.802373	14.813978
20.492801	1012.668092	14.818995
20.522321	1021.395517	14.824013
20.343267	1013.212181	14.829031
20.323203	1002.340642	14.834048
20.237436	1006.882551	14.839066
20.441034	1004.319994	14.844083
20.724749	1008.138513	14.849101
20.159115	1011.164638	14.854119
20.565319	1006.045935	14.859136
20.352507	1007.063717	14.864154
20.546476	1014.998687	14.869171
20.764816	1004.954704	14.874189
20.208148	1012.050352	14.879207
20.411055	1022.830422	14.884224
20.332721	1030.236604	14.889242
20.699046	1028.402933	14.894259
21.038216	1031.963519	14.899277
20.444693	1029.247360	14.904295
20.737951	1025.515834	14.909312
20.588955	1017.242611	14.914330
20.704234	1021.709041	14.919347
20.859544	1024.723905	14.924365
20.561482	1036.459282	14.929383
20.847245	1026.142861	14.934400
20.928960	1031.731657	14.939418
20.838140	1024.806347	14.944435
20.964371	1017.623187	14.949453
20.585103	1009.773978	14.954471
20.820591	1009.222980	14.959488
20.665427	1021.614585	14.964506
20.996746	1021.225388	14.969523
20.938564	1025.709360	14.974541
20.670167	1029.168884	14.979559
20.925075	1021.605932	14.984576
21.109960	1018.446693	14.989594
20.682040	1023.310118	14.994611
21.075815	1015.921204	14.999629
20.956454	1024.422506	15.004647
21.076632	1021.229161	15.009664
20.809832	1021.706249	15.014682
21.156095	1018.985779	15.019699
21.029252	1020.876944	15.024717
20.872577	1030.308694	15.029735
20.974169	1019.427670	15.034752
20.752525	1020.806584	15.039770
20.773683	1029.169247	15.044787
21.273427	1038.836466	15.049805
20.886260	1033.967510	15.054823
20.833257	1039.201748	15.059840
21.243278	1038.626731	15.064858
21.173750	1045.296257	15.069875
21.836307	1037.366876	15.074893
21.686312	1050.527701	15.079911
21.480080	1038.596389	15.084928
21.671981	1042.126258	15.089946
21.169889	1035.122969	15.094963
21.442087	1036.346101	15.099981
21.432927	1039.124646	15.104999
21.935152	1040.201512	15.110016
21.471907	1026.849108	15.115034
21.441966	1015.010282	15.120051
21.490995	1015.053195	15.125069
21.157495	1023.966528	15.130087
21.693653	1027.240826	15.135104
21.724606	1041.004622	15.140122
21.563714	1039.647505	15.145139
21.494169	1041.649669	15.150157
21.704811	1042.090291	15.155175
22.036785	1040.820535	15.160192
21.805883	1023.544067	15.165210
21.974207	1020.826056	15.170227
21.528440	1019.298703	15.175245
21.652127	1021.475904	15.180263
21.702665	1023.626624	15.185280
21.981068	1027.606918	15.190298
21.830346	1031.755011	15.195315
21.612755	1017.120999	15.200333
21.973451	1032.105217	15.205351
22.182702	1030.841947	15.210368
22.052273	1016.405800	15.215386
21.869358	1022.991988	15.220403
21.370038	1019.415423	15.225421
22.217185	1036.851664	15.230439
21.732304	1039.000544	15.235456
21.680822	1041.833016	15.240474
21.944406	1053.020217	15.245491
22.268174	1047.229537	15.250509
22.155404	1041.266989	15.255527
22.460092	1035.826416	15.260544
21.827051	1039.295380	15.265562
21.768410	1046.193582	15.270579
22.109182	1048.690431	15.275597
21.655167	1049.559581	15.280615
21.807253	1050.264936	15.285632
21.877081	1042.673988	15.290650
21.815654	1041.257203	15.295667
22.244249	1057.584691	15.300685
22.662310	1065.285980	15.305703
22.212557	1048.658935	15.310720
22.277237	1048.159776	15.315738
21.956271	1039.266388	15.320755
22.461594	1043.760456	15.325773
22.454446	1056.400435	15.330791
22.207507	1060.090151	15.335808
22.713979	1049.685705	15.340826
22.329988	1061.314559	15.345843
22.536462	1057.489242	15.350861
22.421033	1066.242413	15.355879
22.346271	1069.921102	15.360896
22.361761	1066.977574	15.365914
22.163925	1064.739438	15.370931
22.255190	1057.852037	15.375949
22.320895	1066.198314	15.380967
22.063664	1066.333091	15.385984
22.282299	1067.021774	15.391002
22.784051	1070.759023	15.396019
23.137151	1073.168750	15.401037
22.808410	1072.986462	15.406055
22.787447	1063.055442	15.411072
22.947329	1056.930519	15.416090
22.684376	1061.244413	15.421107
23.172419	1051.385626	15.426125
22.737717	1061.046870	15.431143
22.591948	1054.218465	15.436160
22.823154	1056.255855	15.441178
22.849374	1066.457556	15.446195
22.986807	1067.206218	15.451213
23.025542	1072.243148	15.456231
22.973862	1074.188887	15.461248
23.099631	1073.273123	15.466266
22.949922	1076.887744	15.471283
23.235771	1081.359190	15.476301
22.697974	1071.634865	15.481319
23.133525	1073.198635	15.486336
23.163084	1088.471139	15.491354
23.031876	1088.406416	15.496371
22.907709	1088.788715	15.501389
23.098503	1091.971633	15.506407
23.193639	1088.236227	15.511424
22.913484	1083.590433	15.516442
23.258262	1088.333569	15.521459
23.333541	1082.871897	15.526477
23.583857	1083.858601	15.531495
23.270662	1089.751895	15.536512
23.522234	1080.750408	15.541530
22.988858	1078.416192	15.546547
23.506957	1078.086275	15.551565
23.232982	1075.604375	15.556583
23.433486	1089.060947	15.561600
23.324100	1090.640136	15.566618
23.138771	1084.108210	15.571635
23.282522	1080.125398	15.576653
23.399801	1074.186981	15.581671
23.314378	1083.591887	15.586688
23.720499	1072.243700	15.591706
23.246394	1077.612940	15.596723
23.437706	1078.905472	15.601741
23.680201	1082.291774	15.606759
23.509732	1088.762441	15.611776
23.435900	1074.345838	15.616794
23.161839	1086.348907	15.621811
23.774164	1096.869620	15.626829
23.899682	1107.563962	15.631847
23.729447	1112.712334	15.636864
23.984503	1105.714206	15.641882
23.852740	1105.479158	15.646899
23.962593	1101.362766	15.651917
24.219552	1106.368885	15.656935
23.997270	1087.014518	15.661952
23.641062	1077.678478	15.666970
24.103858	1090.548266	15.671987
23.925433	1085.586835	15.677005
23.949487	1077.479143	15.682023
23.846954	1078.381930	15.687040
23.997552	1088.261325	15.692058
23.738772	1089.352540	15.697075
24.173515	1099.799919	15.702093
23.926043	1092.160524	15.707111
23.971555	1098.382974	15.712128
24.005875	1097.939033	15.717146
24.151424	1104.672924	15.722163
24.174329	1095.230512	15.727181
24.046142	1095.745979	15.732199
23.734942	1106.833361	15.737216
24.269738	1097.465881	15.742234
23.954317	1099.263339	15.747251
24.055944	1100.064914	15.752269
24.008862	1095.376517	15.757287
23.919427	1109.389481	15.762304
24.416294	1117.135328	15.767322
24.545531	1130.647208	15.772339
24.015670	1132.171947	15.777357
24.811316	1125.746045	15.782375
24.671925	1129.655713	15.787392
24.880279	1120.367448	15.792410
24.470505	1114.129230	15.797427
24.095056	1114.007861	15.802445
24.655792	1112.147068	15.807463
24.857459	1123.066246	15.812480
24.622669	1116.762912	15.817498
24.452416	1126.644947	15.822515
24.905870	1123.598507	15.827533
24.809475	1123.758735	15.832551
24.612948	1124.666692	15.837568
24.877604	1113.425710	15.842586
24.630961	1119.933495	15.847603
24.646104	1121.316574	15.852621
24.919929	1118.866142	15.857639
25.245070	1119.740213	15.862656
25.029165	1110.912481	15.867674
24.421928	1101.205263	15.872691
24.494621	1103.052746	15.877709
24.911611	1119.104389	15.882727
24.928365	1122.390148	15.887744
24.851587	1123.904303	15.892762
24.934462	1122.477668	15.897779
24.705587	1123.355948	15.902797
25.219982	1118.693733	15.907815
24.874595	1130.007356	15.912832
24.988325	1111.730412	15.917850
25.150404	1120.011217	15.922867
24.814516	1121.086038	15.927885
24.831028	1118.448452	15.932903
24.594218	1130.496243	15.937920
24.930881	1126.694823	15.942938
25.016954	1131.049064	15.947955
25.423681	1146.906673	15.952973
25.545315	1148.923264	15.957991
25.321960	1129.146144	15.963008
25.702310	1123.848397	15.968026
25.408973	1118.857512	15.973043
25.082609	1120.533602	15.978061
25.432243	1119.630316	15.983079
25.474127	1135.888699	15.988096
25.816187	1134.327036	15.993114
25.606167	1123.554425	15.998131
25.267205	1123.297988	16.003149
25.680270	1121.782075	16.008167
25.439899	1116.170724	16.013184
25.649542	1109.858156	16.018202
25.414593	1118.396434	16.023219
25.242251	1125.833072	16.028237
25.940768	1134.664673	16.033255
25.490441	1139.673627	16.038272
25.634961	1131.805927	16.043290
25.595326	1144.694022	16.048307
25.513885	1137.590484	16.053325
25.975815	1138.531621	16.058343
25.640523	1144.390504	16.063360
25.586834	1134.331997	16.068378
25.538997	1143.970922	16.073395
25.701443	1141.481024	16.078413
26.003301	1134.450352	16.083431
25.848775	1140.858595	16.088448
25.814005	1135.470845	16.093466
25.916015	1137.430531	16.098483
25.804621	1133.197102	16.103501
26.014751	1133.173906	16.108519
25.837772	1134.716287	16.113536
26.134882	1142.095618	16.118554
26.045157	1149.421573	16.123571
25.958432	1153.313579	16.128589
26.369448	1157.819204	16.133607
26.329695	1159.621085	16.138624
26.131019	1151.794187	16.143642
26.123225	1139.024033	16.148659
26.004096	1157.308264	16.153677
26.285331	1152.003851	16.158695
26.158902	1166.518077	16.163712
26.120709	1157.937205	16.168730
26.451538	1162.392200	16.173747
25.689127	1162.037592	16.178765
26.388177	1150.795225	16.183783
26.296640	1154.482855	16.188800
26.325886	1161.197005	16.193818
26.732976	1150.912115	16.198835
26.430110	1167.325187	16.203853
26.431246	1153.142998	16.208871
26.358026	1152.453870	16.213888
26.545800	1155.062918	16.218906
26.738471	1147.875673	16.223923
26.525342	1151.437068	16.228941
26.872013	1143.007718	16.233959
26.466513	1152.137450	16.238976
26.886416	1149.339224	16.243994
26.715747	1148.728384	16.249011
26.600903	1153.101290	16.254029
26.988205	1148.430454	16.259047
27.062321	1152.773939	16.264064
27.006487	1156.831548	16.269082
26.830149	1152.390477	16.274099
26.678690	1154.585287	16.279117
26.787112	1143.296029	16.284135
26.957495	1154.198007	16.289152
26.804883	1158.059247	16.294170
26.987721	1166.267415	16.299187
27.179174	1179.889565	16.304205
27.004762	1164.548126	16.309223
27.119847	1171.545559	16.314240
27.244639	1175.152174	16.319258
27.220495	1173.294077	16.324275
26.716347	1165.031900	16.329293
27.069832	1160.277964	16.334311
26.847991	1168.444999	16.339328
26.968571	1172.784411	16.344346
27.040666	1167.285339	16.349363
26.878880	1178.172778	16.354381
26.980753	1173.786215	16.359399
27.052720	1162.347987	16.364416
27.101078	1180.823914	16.369434
27.379525	1190.926456	16.374451
27.459322	1191.813484	16.379469
27.450248	1189.078886	16.384487
27.688379	1188.600055	16.389504
27.493375	1199.700960	16.394522
27.810991	1189.142802	16.399539
27.903426	1190.602215	16.404557
27.631624	1183.121202	16.409575
27.680582	1183.094698	16.414592
27.589636	1174.705067	16.419610
27.333251	1191.505397	16.424627
27.367499	1197.827465	16.429645
27.481762	1193.868155	16.434663
28.052900	1195.148895	16.439680
27.861315	1194.282535	16.444698
27.983541	1194.478152	16.449715
27.561111	1196.450071	16.454733
27.922329	1195.030586	16.459751
27.845361	1187.522392	16.464768
27.681124	1184.512154	16.469786
28.215938	1191.365350	16.474803
27.555415	1199.774269	16.479821
28.090931	1195.821953	16.484839
28.040186	1191.837841	16.489856
27.748805	1195.957379	16.494874
28.229978	1197.728650	16.499891
27.809168	1203.294756	16.504909
28.022967	1197.006757	16.509927
28.069189	1193.480915	16.514944
27.928600	1196.150561	16.519962
28.276931	1202.777177	16.524979
28.501050	1209.388422	16.529997
28.407661	1201.185350	16.535015
28.231899	1202.639184	16.540032
28.159755	1202.786170	16.545050
28.356640	1203.197379	16.550067
28.559329	1205.671569	16.555085
28.227126	1199.790469	16.560103
28.060136	1204.850001	16.565120
28.375412	1223.754627	16.570138
28.492791	1207.155897	16.575155
28.355454	1217.421019	16.580173
28.506138	1226.921783	16.585191
28.458050	1220.185402	16.590208
28.369616	1214.462003	16.595226
28.803382	1215.347569	16.600243
28.376466	1227.141003	16.605261
28.536632	1225.156374	16.610279
28.642629	1218.503301	16.615296
28.348572	1214.516042	16.620314
28.414514	1211.283770	16.625331
28.742376	1212.065905	16.630349
28.679594	1217.200733	16.635367
28.832258	1233.211583	16.640384
28.768026	1241.246816	16.645402
29.353641	1240.710725	16.650419
29.352149	1229.646807	16.655437
29.014501	1225.467518	16.660455
28.793558	1208.763673	16.665472
28.974261	1213.128447	16.670490
29.126122	1206.392499	16.675507
29.145410	1211.019088	16.680525
29.053096	1210.064689	16.685543
28.999029	1214.431303	16.690560
29.283744	1231.014880	16.695578
29.726499	1236.572774	16.700595
29.524039	1225.836793	16.705613
29.154165	1214.760813	16.710631
29.218932	1218.578753	16.715648
29.441047	1215.315854	16.720666
29.472917	1207.809640	16.725683
29.300199	1209.796329	16.730701
29.300616	1206.236591	16.735719
29.720528	1208.560197	16.740736
29.369520	1210.378986	16.745754
29.469975	1212.247404	16.750771
29.498091	1206.909801	16.755789
29.469081	1203.032755	16.760807
29.370587	1203.969634	16.765824
29.263270	1219.348768	16.770842
29.618524	1214.910121	16.775859
29.489330	1229.181832	16.780877
29.881611	1234.002817	16.785895
29.684641	1223.183933	16.790912
29.914844	1235.787085	16.795930
29.816557	1225.842767	16.800947
29.940931	1227.297210	16.805965
29.997110	1232.271510	16.810983
29.750406	1235.042890	16.816000
29.680262	1238.878684	16.821018
29.969687	1233.869616	16.826035
29.718255	1238.620414	16.831053
29.395164	1238.011211	16.836071
29.597110	1233.214578	16.841088
29.644955	1237.338114	16.846106
29.919760	1228.029980	16.851123
29.675075	1233.814825	16.856141
30.114512	1247.931746	16.861159
30.541775	1252.646304	16.866176
30.214157	1254.890644	16.871194
30.356123	1242.952318	16.876211
30.030525	1249.062189	16.881229
30.113949	1248.680027	16.886247
30.313066	1251.038015	16.891264
30.217327	1256.076999	16.896282
30.612462	1249.640828	16.901299
30.775847	1251.900238	16.906317
30.418383	1252.956335	16.911335
30.750175	1247.167497	16.916352
30.302675	1241.588356	16.921370
30.080446	1237.066047	16.926387
30.641172	1251.710039	16.931405
30.659478	1259.584106	16.936423
30.792771	1248.114184	16.941440
30.917724	1264.435490	16.946458
30.424526	1246.218191	16.951475
30.405267	1243.986942	16.956493
30.336539	1248.409495	16.961511
30.616876	1247.264530	16.966528
30.345676	1253.097691	16.971546
30.557020	1248.735090	16.976563
30.693042	1249.752222	16.981581
30.685579	1258.536014	16.986599
30.820390	1240.826854	16.991616
30.740972	1251.035641	16.996634
30.776735	1247.066450	17.001651
30.834015	1261.801458	17.006669
30.939216	1265.288066	17.011687
31.387148	1259.856681	17.016704
31.238293	1277.558687	17.021722
31.539168	1261.616145	17.026739
31.094262	1251.059908	17.031757
30.947196	1250.445389	17.036775
30.972734	1255.178314	17.041792
31.087602	1264.324914	17.046810
31.309406	1265.959850	17.051827
31.271602	1262.365026	17.056845
31.603398	1268.962684	17.061863
31.646111	1266.901664	17.066880
31.367815	1262.145082	17.071898
31.528237	1263.284647	17.076915
31.566076	1259.435050	17.081933
31.326416	1261.574179	17.086951
31.293166	1264.466963	17.091968
31.133058	1261.736935	17.096986
31.370147	1262.924524	17.102003
31.099634	1254.562813	17.107021
30.870332	1256.280607	17.112039
31.261436	1271.152995	17.117056
31.399109	1284.890896	17.122074
31.355010	1277.866696	17.127091
31.826209	1263.715373	17.132109
31.819439	1283.929367	17.137127
32.071389	1278.679969	17.142144
31.902917	1279.861276	17.147162
31.811324	1286.218748	17.152179
32.072666	1282.479515	17.157197
31.910314	1288.510334	17.162215
31.839502	1288.767565	17.167232
32.088753	1291.266076	17.172250
31.976980	1284.151423	17.177267
31.944138	1286.226795	17.182285
32.218313	1282.671756	17.187303
32.161405	1282.251482	17.192320
32.174709	1281.331127	17.197338
31.954770	1284.827337	17.202355
32.321561	1288.942251	17.207373
32.320099	1284.442361	17.212391
32.294655	1287.744188	17.217408
32.079889	1284.953239	17.222426
32.115547	1285.253854	17.227443
32.059442	1286.859478	17.232461
31.950069	1295.024839	17.237479
32.390454	1299.992987	17.242496
32.650971	1307.946129	17.247514
32.654966	1305.562929	17.252531
32.639561	1309.936171	17.257549
32.660509	1312.953068	17.262567
32.785586	1304.889503	17.267584
32.539322	1301.860459	17.272602
32.526828	1310.452556	17.277619
32.519847	1314.852888	17.282637
32.682953	1314.685536	17.287655
32.527199	1312.645944	17.292672
32.689326	1311.658235	17.297690
32.527335	1307.565186	17.302707
32.740084	1306.591686	17.307725
32.519075	1308.595372	17.312743
32.976174	1305.346363	17.317760
32.995200	1304.090601	17.322778
32.498043	1304.246955	17.327795
32.708788	1313.691077	17.332813
32.968443	1331.487323	17.337831
33.148532	1324.696442	17.342848
33.276607	1326.658402	17.347866
33.379739	1327.024252	17.352883
33.751178	1321.633160	17.357901
33.174294	1314.827597	17.362919
33.223007	1296.708909	17.367936
33.156077	1301.591943	17.372954
33.252641	1297.575405	17.377971
33.571191	1292.003208	17.382989
33.213570	1305.325936	17.388007
33.453237	1306.487880	17.393024
33.629417	1316.275056	17.398042
33.458722	1314.850016	17.403059
33.215738	1305.044948	17.408077
33.559451	1324.131446	17.413095
33.779710	1314.762332	17.418112
33.942911	1323.806763	17.423130
33.829422	1313.924723	17.428147
33.478952	1294.571153	17.433165
33.411792	1304.613960	17.438183
33.763495	1309.857850	17.443200
33.677455	1313.225921	17.448218
33.984202	1322.718216	17.453235
34.003968	1312.291566	17.458253
33.730230	1320.842292	17.463271
33.720304	1319.597348	17.468288
33.925586	1318.606075	17.473306
33.802226	1316.504635	17.478323
34.003907	1318.016477	17.483341
33.699251	1322.393731	17.488359
33.880018	1318.307273	17.493376
33.898133	1324.641366	17.498394
33.905572	1327.761355	17.503411
34.062978	1317.205975	17.508429
33.983481	1330.987192	17.513447
34.006082	1341.378962	17.518464
34.358522	1344.722950	17.523482
34.386251	1341.442956	17.528499
34.292740	1334.331751	17.533517
34.358032	1350.561439	17.538535
34.090956	1343.650824	17.543552
34.378373	1349.718934	17.548570
34.108121	1348.946866	17.553587
34.108204	1350.969782	17.558605
34.361165	1352.890210	17.563623
34.452808	1354.444434	17.568640
34.255596	1350.293743	17.573658
34.321874	1360.918565	17.578675
34.619872	1368.471422	17.583693
34.714924	1364.489819	17.588711
34.409781	1373.468338	17.593728
34.496913	1370.586190	17.598746
34.586306	1369.161676	17.603763
34.762634	1367.761497	17.608781
34.620844	1373.893286	17.613799
34.851074	1371.288660	17.618816
35.031840	1371.266881	17.623834
34.708828	1372.188232	17.628851
35.262716	1372.335578	17.633869
35.036743	1371.231566	17.638887
34.837101	1367.239039	17.643904
34.831674	1363.620219	17.648922
35.326781	1382.847311	17.653939
35.500977	1373.535831	17.658957
35.091244	1376.569302	17.663975
35.350043	1364.467536	17.668992
35.317373	1361.070710	17.674010
35.320537	1374.021734	17.679027
35.480292	1376.502633	17.684045
35.443805	1366.640133	17.689063
35.390595	1369.289889	17.694080
35.362975	1374.381417	17.699098
35.368016	1395.114408	17.704115
35.708292	1391.388109	17.709133
35.609771	1398.567213	17.714151
35.692999	1390.033596	17.719168
35.769690	1388.595280	17.724186
35.456931	1394.643241	17.729203
35.375043	1390.988983	17.734221
35.993891	1392.388543	17.739239
35.910944	1384.653977	17.744256
36.055589	1382.962083	17.749274
35.791403	1390.987489	17.754291
36.115724	1378.155987	17.759309
35.831807	1388.472431	17.764327
35.673395	1391.529891	17.769344
35.954145	1387.011282	17.774362
35.730993	1383.678823	17.779379
35.991364	1377.194160	17.784397
35.744390	1383.907219	17.789415
36.158684	1383.823835	17.794432
36.384574	1386.698382	17.799450
35.813586	1390.514358	17.804467
36.144392	1381.588747	17.809485
36.201750	1390.829573	17.814503
36.004175	1405.560198	17.819520
36.333295	1403.426168	17.824538
36.189172	1417.640394	17.829555
36.571192	1403.275627	17.834573
36.269661	1413.784177	17.839591
36.478441	1412.211684	17.844608
36.736397	1411.625618	17.849626
36.602449	1412.751065	17.854643
36.949898	1413.697418	17.859661
36.759453	1405.834413	17.864679
36.636447	1414.983412	17.869696
36.775256	1398.046650	17.874714
36.837922	1408.634194	17.879731
36.772209	1411.936002	17.884749
36.826219	1410.996679	17.889767
36.787703	1405.833494	17.894784
37.000856	1415.384593	17.899802
36.792775	1415.663198	17.904819
36.948492	1411.053597	17.909837
37.180405	1409.360737	17.914855
36.983982	1406.402810	17.919872
37.174967	1398.338409	17.924890
36.949342	1410.845397	17.929907
37.256482	1398.840224	17.934925
37.409845	1410.903195	17.939943
37.050995	1410.432098	17.944960
37.135443	1408.433992	17.949978
37.265100	1407.236737	17.954995
36.992203	1403.413399	17.960013
37.445232	1413.024980	17.965031
37.187917	1404.743194	17.970048
37.352402	1399.901856	17.975066
37.360844	1413.618952	17.980083
37.173976	1404.369984	17.985101
37.307970	1413.084491	17.990119
37.235366	1413.932142	17.995136
37.432709	1421.349214	18.000154
37.464578	1420.899335	18.005171
37.639986	1430.528902	18.010189
38.157741	1429.684634	18.015207
38.099580	1430.271260	18.020224
37.913771	1424.029619	18.025242
37.837814	1421.327490	18.030259
37.741418	1413.787511	18.035277
37.918302	1420.251554	18.040295
37.969987	1420.972556	18.045312
38.042939	1411.632638	18.050330
38.315476	1423.333078	18.055347
37.680658	1415.296257	18.060365
38.218953	1405.416829	18.065383
37.964456	1417.344490	18.070400
38.200038	1409.383594	18.075418
38.097049	1412.893178	18.080435
38.263908	1417.190730	18.085453
38.406812	1415.991412	18.090471
37.768726	1420.900289	18.095488
38.340757	1401.870034	18.100506
38.158766	1416.831773	18.105523
38.109002	1404.257312	18.110541
38.500013	1414.216222	18.115559
38.465227	1428.511264	18.120576
38.629138	1435.501199	18.125594
38.907911	1420.205746	18.130611
38.907890	1423.718235	18.135629
39.031151	1400.494335	18.140647
39.030685	1396.991501	18.145664
39.000364	1394.238089	18.150682
38.766251	1399.150335	18.155699
38.614955	1398.438640	18.160717
38.578982	1398.870330	18.165735
38.438969	1406.355700	18.170752
38.636166	1405.949508	18.175770
38.858154	1416.206136	18.180787
38.948216	1412.809126	18.185805
39.554034	1406.964949	18.190823
39.119324	1416.781021	18.195840
39.351526	1414.942947	18.200858
39.361592	1412.167465	18.205875
39.317447	1407.794111	18.210893
39.375776	1407.191789	18.215911
39.056400	1411.508240	18.220928
39.166486	1406.943615	18.225946
39.309388	1413.226752	18.230963
38.983432	1417.247582	18.235981
39.478085	1411.767851	18.240999
39.169301	1415.410464	18.246016
39.333061	1407.751087	18.251034
39.277974	1419.493067	18.256051
39.003931	1421.161037	18.261069
39.663658	1429.269831	18.266087
39.455971	1436.658452	18.271104
39.851450	1430.638731	18.276122
40.044134	1445.030915	18.281139
39.869312	1448.428613	18.286157
39.964687	1443.591711	18.291175
39.789038	1432.406459	18.296192
39.981441	1439.029040	18.301210
39.958261	1442.715554	18.306227
39.748364	1448.753829	18.311245
39.912857	1432.365306	18.316263
39.792491	1441.999906	18.321280
39.579474	1440.180655	18.326298
39.942038	1439.960156	18.331315
40.020972	1441.942403	18.336333
40.066141	1438.606027	18.341351
40.342330	1447.494072	18.346368
40.109201	1438.258601	18.351386
40.226231	1436.255419	18.356403
40.279769	1456.984087	18.361421
40.508012	1455.377001	18.366439
40.268770	1459.220236	18.371456
40.399606	1459.515502	18.376474
40.613842	1453.022216	18.381491
40.361172	1453.812697	18.386509
40.723104	1454.431747	18.391527
40.375364	1469.968452	18.396544
40.479573	1462.419310	18.401562
40.561216	1454.498140	18.406579
40.297424	1455.101003	18.411597
40.594915	1458.131674	18.416615
40.630471	1464.620893	18.421632
40.875879	1473.974496	18.426650
41.064098	1474.011517	18.431667
41.052535	1480.953051	18.436685
41.060989	1481.403073	18.441703
41.211380	1478.905537	18.446720
41.084832	1482.103220	18.451738
41.230828	1480.493158	18.456755
41.159031	1492.326151	18.461773
41.449652	1481.967685	18.466791
41.262187	1479.885673	18.471808
41.267377	1481.948835	18.476826
40.942038	1478.960474	18.481843
41.195019	1479.362957	18.486861
41.009555	1470.075866	18.491879
40.791073	1481.104861	18.496896
41.028114	1480.061298	18.501914
41.408529	1485.376510	18.506931
41.350905	1502.404964	18.511949
41.664589	1491.212917	18.516967
41.547433	1508.951242	18.521984
41.594038	1506.160590	18.527002
41.839395	1494.682529	18.532019
41.619594	1495.531012	18.537037
41.721955	1495.524596	18.542055
41.705262	1503.539922	18.547072
41.556559	1500.842795	18.552090
41.921481	1497.194689	18.557107
42.064891	1500.116811	18.562125
41.761348	1491.987351	18.567143
41.936702	1510.065147	18.572160
42.053019	1517.823082	18.577178
42.197326	1527.283974	18.582195
42.080846	1529.782655	18.587213
42.634778	1517.495979	18.592231
42.295986	1526.025372	18.597248
42.308458	1517.155569	18.602266
42.610604	1520.283357	18.607283
42.314415	1527.991911	18.612301
42.425562	1520.454288	18.617319
42.572163	1522.549086	18.622336
42.582942	1519.416867	18.627354
42.533060	1517.969844	18.632371
42.432732	1514.870704	18.637389
42.972450	1518.621073	18.642407
42.685741	1512.710695	18.647424
42.603293	1518.927969	18.652442
42.826112	1514.500400	18.657459
42.832262	1525.112592	18.662477
42.758707	1523.798644	18.667495
42.821346	1520.986558	18.672512
42.508901	1518.052988	18.677530
42.412906	1515.473887	18.682547
42.153381	1523.773185	18.687565
42.409558	1535.946467	18.692583
42.691472	1545.783580	18.697600
43.147269	1548.177384	18.702618
43.320108	1547.576164	18.707635
43.271193	1548.252873	18.712653
43.183191	1538.019597	18.717671
43.492162	1548.007135	18.722688
43.241999	1550.826440	18.727706
43.344106	1548.551009	18.732723
43.424937	1555.929473	18.737741
43.585723	1554.651622	18.742759
43.749498	1565.340283	18.747776
43.629106	1564.339742	18.752794
43.637444	1563.098249	18.757811
43.589454	1566.198507	18.762829
43.621401	1570.722232	18.767847
43.853729	1562.446190	18.772864
43.869062	1564.946445	18.777882
44.215347	1569.743125	18.782899
43.599936	1574.124641	18.787917
43.798903	1568.908654	18.792935
44.015642	1574.722755	18.797952
43.876661	1566.034300	18.802970
43.792341	1563.604855	18.807987
43.936457	1572.380980	18.813005
44.214823	1561.759285	18.818023
44.265121	1571.452590	18.823040
43.850629	1568.585394	18.828058
44.190723	1565.679608	18.833075
44.245892	1569.903068	18.838093
43.778711	1574.996818	18.843111
44.256179	1587.034694	18.848128
44.077330	1589.293783	18.853146
44.187338	1590.444375	18.858163
44.380943	1590.613104	18.863181
44.412208	1583.466594	18.868199
44.452106	1583.409942	18.873216
44.539640	1605.796625	18.878234
44.443748	1609.204155	18.883251
44.845433	1616.857741	18.888269
44.892233	1609.405840	18.893287
45.256961	1609.364886	18.898304
45.148058	1610.593745	18.903322
45.310664	1607.387378	18.908339
45.277035	1593.301772	18.913357
45.130325	1580.417227	18.918375
45.192936	1576.166068	18.923392
44.870698	1586.829425	18.928410
45.386272	1584.404408	18.933427
45.010411	1580.325659	18.938445
45.282271	1586.563532	18.943463
45.349479	1591.492033	18.948480
45.283821	1602.582518	18.953498
45.570918	1595.011157	18.958515
45.282386	1592.739737	18.963533
45.116685	1597.754996	18.968551
45.503888	1600.405644	18.973568
45.514073	1601.666455	18.978586
45.630292	1600.010525	18.983603
45.251337	1601.691690	18.988621
45.382432	1598.269321	18.993639
45.868077	1597.168109	18.998656
45.883506	1596.272654	19.003674
45.718794	1595.036011	19.008691
45.586068	1601.822884	19.013709
45.618935	1595.745954	19.018727
45.531802	1598.940677	19.023744
45.792520	1609.090399	19.028762
45.965010	1615.173338	19.033779
46.018687	1626.014879	19.038797
45.796791	1621.429302	19.043815
46.110164	1621.128097	19.048832
46.009850	1634.019680	19.053850
45.990235	1631.214071	19.058867
46.339903	1623.910672	19.063885
46.362909	1633.283206	19.068903
46.436010	1646.296125	19.073920
46.765477	1652.263115	19.078938
46.645015	1640.289642	19.083955
46.504612	1634.870849	19.088973
46.908873	1632.466312	19.093991
46.721469	1633.454926	19.099008
46.977559	1632.783936	19.104026
46.728061	1625.718993	19.109043
46.704322	1624.324696	19.114061
46.663772	1630.917345	19.119079
47.109353	1634.748669	19.124096
46.993588	1640.084375	19.129114
47.136012	1638.790442	19.134131
47.033657	1649.353328	19.139149
46.817662	1648.774774	19.144167
47.266414	1646.050877	19.149184
47.171294	1647.056682	19.154202
47.317039	1643.180735	19.159219
46.996301	1640.153760	19.164237
46.995850	1642.817432	19.169255
47.043269	1636.694041	19.174272
47.130512	1636.377549	19.179290
47.437896	1639.084813	19.184307
47.362990	1643.031890	19.189325
47.532244	1650.462899	19.194343
47.881337	1661.832835	19.199360
47.401589	1656.788768	19.204378
47.803447	1660.263981	19.209395
47.868904	1662.286221	19.214413
47.598671	1666.352080	19.219431
47.909290	1664.940437	19.224448
47.748926	1665.899596	19.229466
47.702541	1666.216147	19.234483
47.800174	1668.832993	19.239501
47.719339	1667.974613	19.244519
47.975774	1661.916503	19.249536
47.832165	1665.255732	19.254554
47.875887	1664.175984	19.259571
47.953575	1666.521375	19.264589
48.056113	1680.694251	19.269607
48.593706	1680.181405	19.274624
48.244403	1694.329965	19.279642
48.625472	1690.246951	19.284659
48.557082	1688.638691	19.289677
48.447433	1688.150878	19.294695
48.762028	1678.362934	19.299712
48.259314	1687.201955	19.304730
48.292823	1682.406180	19.309747
48.643410	1681.392264	19.314765
48.372247	1692.868258	19.319783
48.718165	1686.237618	19.324800
48.793714	1685.168693	19.329818
48.994197	1683.553285	19.334835
48.713659	1685.578905	19.339853
48.339650	1688.890893	19.344871
48.965732	1689.367838	19.349888
49.090823	1703.085930	19.354906
49.280125	1711.230226	19.359923
49.058245	1708.954725	19.364941
49.150778	1711.307278	19.369959
49.363730	1712.101016	19.374976
49.300016	1707.976793	19.379994
49.317936	1713.635698	19.385011
49.497087	1708.754122	19.390029
49.242456	1713.868469	19.395047
49.737356	1708.805186	19.400064
49.026264	1713.091177	19.405082
49.179886	1707.563466	19.410099
49.659565	1704.525470	19.415117
49.519176	1705.910720	19.420135
49.717019	1705.731644	19.425152
49.483850	1705.310400	19.430170
49.818087	1728.454106	19.435187
49.956533	1725.718550	19.440205
49.883624	1732.934826	19.445223
49.593016	1727.750835	19.450240
49.745133	1735.276068	19.455258
49.913810	1743.010169	19.460275
50.283193	1734.958867	19.465293
50.033094	1739.769551	19.470311
50.193909	1733.956683	19.475328
50.032323	1738.425374	19.480346
50.167378	1725.168644	19.485363
50.384221	1744.246943	19.490381
50.209154	1753.457871	19.495399
50.523117	1752.629539	19.500416
50.326104	1757.021698	19.505434
50.290573	1760.410391	19.510451
50.508504	1758.940587	19.515469
50.285346	1760.714278	19.520487
50.861517	1757.405623	19.525504
50.551747	1757.428660	19.530522
50.320867	1757.556181	19.535539
50.780931	1770.893960	19.540557
51.056448	1779.662353	19.545575
51.222778	1770.942042	19.550592
51.168498	1767.390708	19.555610
51.230934	1767.125414	19.560627
51.535889	1765.945025	19.565645
51.201420	1772.848583	19.570663
51.364092	1763.538694	19.575680
51.480635	1760.386810	19.580698
51.431483	1763.458880	19.585715
51.551201	1761.221708	19.590733
51.394422	1756.714323	19.595751
51.566505	1762.551216	19.600768
51.285048	1764.911511	19.605786
51.505607	1765.451596	19.610803
51.727316	1762.624173	19.615821
51.764065	1762.460711	19.620839
51.831829	1755.813391	19.625856
51.971631	1767.247538	19.630874
51.609731	1761.071066	19.635891
51.855799	1761.443074	19.640909
51.624244	1760.778573	19.645927
52.090557	1751.370921	19.650944
52.217375	1759.076833	19.655962
51.866795	1754.615401	19.660979
51.680100	1755.673340	19.665997
51.874825	1764.725711	19.671015
52.337441	1773.180941	19.676032
52.424861	1782.344704	19.681050
52.769676	1784.342399	19.686067
52.713738	1767.012720	19.691085
51.984363	1765.968124	19.696103
52.367218	1769.010805	19.701120
52.565223	1767.872315	19.706138
52.486342	1775.708092	19.711155
52.682712	1773.140239	19.716173
52.332614	1783.950066	19.721191
52.388329	1776.831230	19.726208
52.546621	1773.079537	19.731226
52.466742	1784.405884	19.736243
52.796101	1786.121955	19.741261
53.093108	1807.892438	19.746279
53.174376	1806.926760	19.751296
53.054621	1812.332568	19.756314
52.816080	1808.333375	19.761331
52.972849	1801.003131	19.766349
52.891449	1804.048670	19.771367
53.028579	1798.608708	19.776384
53.049017	1792.183343	19.781402
53.037525	1805.818635	19.786419
53.824869	1807.049981	19.791437
53.931437	1818.726028	19.796455
54.127318	1809.019615	19.801472
53.910458	1796.480361	19.806490
53.729905	1789.095341	19.811507
53.836675	1777.291529	19.816525
54.096964	1782.341504	19.821543
54.245107	1780.516481	19.826560
54.209291	1783.191992	19.831578
54.230322	1777.075817	19.836595
54.119214	1779.071912	19.841613
53.639939	1789.504212	19.846631
53.975875	1787.044019	19.851648
53.570824	1778.497875	19.856666
54.165243	1797.040905	19.861683
54.510725	1802.623590	19.866701
54.351292	1809.402077	19.871719
54.355113	1813.349558	19.876736
54.435582	1812.273547	19.881754
54.488683	1811.025068	19.886771
54.344499	1811.019167	19.891789
54.707148	1820.301049	19.896807
54.512926	1819.100543	19.901824
54.733943	1803.135238	19.906842
54.568715	1811.675615	19.911859
54.429221	1809.339935	19.916877
54.551933	1812.227461	19.921895
54.001649	1818.325169	19.926912
54.767710	1821.964622	19.931930
54.424336	1831.498449	19.936947
54.682520	1824.736246	19.941965
55.105807	1837.940941	19.946983
55.094547	1846.624625	19.952000
55.217357	1847.823736	19.957018
55.170627	1858.867249	19.962035
55.132112	1859.889500	19.967053
55.210730	1860.808305	19.972071
55.490936	1857.861303	19.977088
55.676509	1861.723691	19.982106
55.470430	1861.162521	19.987123
55.646356	1856.757948	19.992141
55.561250	1855.461554	19.997159
55.619968	1857.295512	20.002176
55.546168	1854.324730	20.007194
55.114170	1857.576348	20.012211
55.947275	1867.293106	20.017229
55.877708	1874.442645	20.022247
56.080177	1879.126097	20.027264
56.543249	1868.529113	20.032282
56.235295	1866.610986	20.037299
56.291728	1853.145489	20.042317
56.288845	1846.357651	20.047335
56.402531	1845.936050	20.052352
56.464873	1836.461858	20.057370
56.249949	1842.693559	20.062387
56.641219	1850.288906	20.067405
56.589389	1869.181945	20.072423
56.500581	1864.818589	20.077440
56.600860	1859.163433	20.082458
56.526252	1856.953348	20.087475
56.636498	1862.342297	20.092493
56.585235	1866.427758	20.097511
56.574875	1867.332014	20.102528
56.817566	1861.862973	20.107546
56.705534	1865.064776	20.112563
56.517920	1866.668836	20.117581
56.773927	1879.861736	20.122599
57.009862	1884.060282	20.127616
56.949364	1881.832218	20.132634
57.198448	1889.645385	20.137651
57.466756	1888.921989	20.142669
57.371895	1884.913032	20.147687
57.052757	1892.754708	20.152704
57.441752	1881.828411	20.157722
57.584626	1883.494630	20.162739
57.352117	1888.785468	20.167757
57.476059	1890.713420	20.172775
57.554289	1910.996944	20.177792
57.736517	1910.230143	20.182810
57.738107	1913.086049	20.187827
57.915196	1918.537193	20.192845
57.550475	1920.758988	20.197863
57.703430	1917.860192	20.202880
57.834736	1911.256571	20.207898
57.846925	1917.055292	20.212915
57.636080	1926.448610	20.217933
58.095191	1923.568420	20.222951
57.934997	1935.920416	20.227968
58.244316	1933.726288	20.232986
58.308236	1945.027192	20.238003
58.405971	1933.136319	20.243021
58.541999	1939.950906	20.248039
58.167646	1941.991160	20.253056
58.587543	1942.336107	20.258074
58.722845	1948.251375	20.263091
58.636608	1948.574136	20.268109
59.023062	1953.418317	20.273127
58.695400	1959.714949	20.278144
59.094788	1954.928410	20.283162
58.625340	1959.142120	20.288179
59.100784	1957.143039	20.293197
58.890320	1955.515848	20.298215
58.962770	1961.081131	20.303232
59.290501	1954.326987	20.308250
59.112720	1961.897367	20.313267
59.044171	1948.422854	20.318285
59.345091	1960.677826	20.323303
59.006521	1955.457053	20.328320
59.022022	1953.564299	20.333338
59.271682	1972.195904	20.338355
59.593674	1975.424828	20.343373
59.371799	1975.465738	20.348391
59.617556	1981.606826	20.353408
59.731494	1981.112596	20.358426
59.625764	1976.619298	20.363443
59.786379	1977.632643	20.368461
60.038730	1979.988753	20.373479
59.904366	1982.553401	20.378496
60.172637	1976.143034	20.383514
59.822827	1985.709504	20.388531
59.935291	1991.581003	20.393549
60.349664	2004.263326	20.398567
60.012516	2006.452435	20.403584
59.957834	2000.067095	20.408602
60.246971	1995.083107	20.413619
60.470855	1996.686229	20.418637
60.602187	1998.366879	20.423655
60.556517	1994.681611	20.428672
61.157551	1996.620503	20.433690
60.971147	1988.743987	20.438707
60.792959	1991.145039	20.443725
60.910249	1988.434828	20.448743
60.526121	1989.289982	20.453760
61.202752	1995.360833	20.458778
61.070619	2001.797457	20.463795
61.211929	2015.784674	20.468813
61.315734	2022.525412	20.473831
61.174608	2016.819426	20.478848
61.743173	2003.791651	20.483866
61.472849	2009.280924	20.488883
61.727045	2015.641624	20.493901
61.682038	2006.143030	20.498919
60.786848	2002.287056	20.503936
61.600670	2011.091677	20.508954
61.594872	2007.785222	20.513971
61.170208	2014.715538	20.518989
61.732915	2014.473341	20.524007
61.229909	2015.495333	20.529024
61.824720	2012.149015	20.534042
61.903099	2026.796160	20.539059
62.221330	2040.547559	20.544077
62.083583	2035.560594	20.549095
61.906046	2037.084202	20.554112
62.325427	2037.195692	20.559130
62.564049	2034.324567	20.564147
62.544204	2034.327710	20.569165
62.540678	2032.456845	20.574183
62.093185	2045.301790	20.579200
62.416506	2035.199856	20.584218
62.571555	2029.403570	20.589235
62.592052	2024.783305	20.594253
62.731294	2029.236790	20.599271
62.478088	2030.185176	20.604288
62.453185	2032.183656	20.609306
63.108629	2038.125271	20.614323
62.908653	2044.143267	20.619341
63.033940	2040.185209	20.624359
62.787169	2044.073923	20.629376
63.087726	2039.545756	20.634394
62.920533	2046.019414	20.639411
62.989743	2037.342498	20.644429
63.198972	2029.375963	20.649447
62.991132	2043.215582	20.654464
62.997451	2040.459522	20.659482
63.348820	2057.162885	20.664499
63.372644	2062.767330	20.669517
63.756759	2065.686784	20.674535
63.647495	2067.616348	20.679552
64.010393	2070.453897	20.684570
64.425716	2058.390412	20.689587
63.847211	2069.381145	20.694605
64.089027	2059.913607	20.699623
63.893569	2070.781584	20.704640
64.267908	2063.127012	20.709658
64.242358	2067.274790	20.714675
64.335410	2061.339817	20.719693
64.262660	2061.603673	20.724711
64.130243	2055.142050	20.729728
64.049214	2054.870685	20.734746
64.160302	2054.099175	20.739763
64.144612	2069.505801	20.744781
64.559043	2056.236888	20.749799
64.726268	2057.927735	20.754816
64.317030	2068.393476	20.759834
64.558472	2073.989290	20.764851
64.278540	2087.789673	20.769869
64.834284	2076.064091	20.774887
64.500878	2083.358938	20.779904
64.409848	2088.346928	20.784922
64.926426	2099.829929	20.789939
65.106694	2101.929023	20.794957
65.232069	2109.120891	20.799975
65.137186	2110.489618	20.804992
65.310954	2107.215149	20.810010
65.585846	2107.876180	20.815027
65.222136	2109.753842	20.820045
65.463391	2100.983834	20.825063
65.732122	2116.529264	20.830080
65.525960	2111.410911	20.835098
65.545986	2116.495233	20.840115
65.593948	2129.376712	20.845133
65.659134	2122.341475	20.850151
66.036890	2133.498957	20.855168
66.186483	2136.697945	20.860186
66.360697	2129.756189	20.865203
66.066219	2140.166232	20.870221
66.326577	2132.078076	20.875239
66.393025	2134.056033	20.880256
66.041912	2127.830414	20.885274
66.398201	2129.791647	20.890291
65.760698	2136.764616	20.895309
66.085135	2136.622634	20.900327
66.336138	2142.971253	20.905344
66.145615	2156.142358	20.910362
66.553921	2152.995474	20.915379
66.097806	2164.263869	20.920397
66.702186	2170.014654	20.925415
66.885421	2171.737735	20.930432
67.024799	2174.856266	20.935450
67.425638	2179.597279	20.940467
66.735900	2186.553152	20.945485
67.174233	2173.564467	20.950503
67.429857	2169.393575	20.955520
67.205030	2175.961464	20.960538
67.370657	2178.075470	20.965555
67.456632	2173.691137	20.970573
67.646804	2173.932994	20.975591
67.621808	2169.493353	20.980608
67.684817	2174.290119	20.985626
67.703240	2172.324299	20.990643
67.560095	2181.331651	20.995661
67.824916	2189.107785	21.000679
67.836239	2195.572639	21.005696
67.594434	2192.934086	21.010714
68.234383	2197.637875	21.015731
68.003953	2204.086720	21.020749
68.149829	2194.851811	21.025767
68.218037	2203.993533	21.030784
68.048696	2199.582670	21.035802
68.014411	2203.678189	21.040819
67.949353	2210.991270	21.045837
68.544939	2211.479292	21.050855
68.620990	2216.687470	21.055872
68.195381	2217.356578	21.060890
68.794731	2216.515353	21.065907
68.635929	2224.998119	21.070925
68.802609	2210.265426	21.075943
68.808176	2222.901095	21.080960
68.806236	2216.150842	21.085978
68.930852	2220.590872	21.090995
69.280845	2241.564643	21.096013
69.752537	2242.210818	21.101031
69.805573	2236.613394	21.106048
69.419840	2224.406261	21.111066
69.521804	2211.334213	21.116083
69.562833	2207.957310	21.121101
69.646613	2206.041275	21.126119
69.517772	2216.990491	21.131136
69.467494	2228.927923	21.136154
69.781057	2222.769207	21.141171
69.878405	2231.107947	21.146189
70.031584	2226.713138	21.151207
69.965227	2226.792955	21.156224
69.922800	2229.438002	21.161242
70.121903	2225.070759	21.166259
69.922955	2230.088215	21.171277
69.552981	2226.743740	21.176295
70.196383	2238.229176	21.181312
70.262936	2260.083431	21.186330
70.223547	2258.574751	21.191347
70.229824	2258.466525	21.196365
70.371957	2264.412393	21.201383
70.812522	2255.096855	21.206400
70.283844	2268.955042	21.211418
70.664361	2261.151093	21.216435
70.656908	2278.885725	21.221453
70.771184	2291.403527	21.226471
70.965230	2287.964913	21.231488
70.658935	2287.170010	21.236506
70.721925	2279.399711	21.241523
70.935089	2297.765924	21.246541
71.210654	2306.925910	21.251559
71.345923	2304.380119	21.256576
71.411268	2306.216248	21.261594
71.575891	2299.234892	21.266611
71.773717	2302.981853	21.271629
71.687348	2301.631971	21.276647
71.841787	2299.420886	21.281664
71.956646	2309.278118	21.286682
71.683071	2302.011516	21.291699
71.426717	2306.239468	21.296717
71.710949	2313.450869	21.301735
72.170237	2317.122409	21.306752
71.794487	2329.808055	21.311770
72.401012	2319.766016	21.316787
72.421231	2317.414871	21.321805
72.160017	2328.157534	21.326823
72.719538	2321.102062	21.331840
72.398162	2328.240491	21.336858
72.735465	2314.352200	21.341875
72.871200	2312.585862	21.346893
72.721741	2311.138499	21.351911
72.685962	2318.860500	21.356928
72.904604	2315.806237	21.361946
73.006468	2308.919860	21.366963
73.375330	2311.829106	21.371981
73.379325	2314.788849	21.376999
72.933852	2306.450727	21.382016
72.918015	2323.220978	21.387034
73.188937	2316.245157	21.392051
73.580403	2326.081425	21.397069
73.331430	2342.894305	21.402087
73.705749	2334.037190	21.407104
73.412865	2336.964259	21.412122
73.348003	2339.391897	21.417139
73.532255	2338.454340	21.422157
73.715531	2337.330732	21.427175
73.629239	2326.424513	21.432192
73.539204	2337.320421	21.437210
73.960059	2346.713443	21.442227
74.112118	2356.744801	21.447245
73.839457	2363.026699	21.452263
74.218213	2353.203151	21.457280
74.127082	2366.289503	21.462298
74.634763	2363.783557	21.467315
74.596107	2355.678736	21.472333
74.233085	2365.547283	21.477351
74.582600	2358.865340	21.482368
74.972018	2370.242074	21.487386
74.956991	2369.578554	21.492403
75.225025	2372.017486	21.497421
75.204250	2372.809772	21.502439
75.075629	2354.039085	21.507456
74.902839	2364.206236	21.512474
74.882131	2372.127896	21.517491
75.240519	2378.898563	21.522509
75.295495	2374.339116	21.527527
75.313513	2371.262428	21.532544
75.001683	2374.255573	21.537562
75.321144	2365.078761	21.542579
75.490696	2368.972158	21.547597
75.527138	2390.370485	21.552615
75.649918	2386.526357	21.557632
75.746524	2391.014975	21.562650
75.728537	2394.562012	21.567667
75.934973	2388.577718	21.572685
75.979292	2400.844540	21.577703
75.722370	2385.259261	21.582720
75.962381	2404.643946	21.587738
75.911782	2410.168563	21.592755
75.725150	2403.147175	21.597773
75.911497	2412.980710	21.602791
76.636415	2419.596490	21.607808
76.842145	2424.853970	21.612826
77.094354	2435.444172	21.617843
76.700051	2408.506030	21.622861
76.822572	2430.395963	21.627879
76.914921	2424.596687	21.632896
76.731270	2430.628050	21.637914
77.136075	2429.400514	21.642931
77.247854	2423.629773	21.647949
77.042893	2437.450313	21.652967
77.388675	2433.116990	21.657984
77.091476	2432.910836	21.663002
77.278875	2425.471420	21.668019
77.307740	2432.965641	21.673037
77.262010	2434.733864	21.678055
77.408559	2434.849966	21.683072
77.593416	2453.864571	21.688090
77.471293	2451.794363	21.693107
77.945198	2454.037141	21.698125
77.614195	2461.394887	21.703143
77.930909	2458.574655	21.708160
77.695808	2465.153717	21.713178
78.061468	2469.572061	21.718195
78.279829	2480.337984	21.723213
78.119317	2492.011869	21.728231
78.252806	2485.770639	21.733248
78.635560	2486.771520	21.738266
78.257088	2486.073057	21.743283
78.465851	2475.010349	21.748301
78.681725	2487.335733	21.753319
78.655513	2485.537785	21.758336
78.769856	2502.417332	21.763354
78.871041	2501.170787	21.768371
79.069755	2499.309413	21.773389
78.473218	2502.473147	21.778407
78.799872	2494.519683	21.783424
79.086050	2502.134828	21.788442
79.342983	2512.683312	21.793459
79.736384	2527.865683	21.798477
79.800363	2529.234956	21.803495
80.061466	2522.257428	21.808512
79.690487	2512.335914	21.813530
80.004507	2517.475569	21.818547
79.943390	2518.820134	21.823565
79.838022	2524.264944	21.828583
79.974907	2524.054325	21.833600
79.836248	2523.858202	21.838618
79.809133	2527.498212	21.843635
79.995146	2518.992239	21.848653
80.306200	2528.355111	21.853671
79.748593	2528.435669	21.858688
80.004922	2544.254819	21.863706
80.290978	2554.041348	21.868723
80.474603	2550.310797	21.873741
80.277678	2550.830694	21.878759
80.517788	2559.131580	21.883776
81.017544	2568.449314	21.888794
80.975566	2568.910371	21.893811
80.972355	2575.598547	21.898829
81.106103	2575.467316	21.903847
81.479613	2568.898333	21.908864
81.663160	2568.743568	21.913882
81.144017	2573.943526	21.918899
81.035452	2564.839566	21.923917
81.197813	2576.286499	21.928935
81.470636	2583.695459	21.933952
81.686153	2590.542103	21.938970
81.622687	2594.020517	21.943987
81.964202	2586.699061	21.949005
81.748937	2595.477991	21.954023
82.026429	2590.344163	21.959040
82.118613	2589.793339	21.964058
82.442041	2584.030624	21.969075
82.268607	2582.438637	21.974093
82.191628	2584.309578	21.979111
82.379945	2595.771418	21.984128
82.868604	2614.044567	21.989146
82.451750	2612.525193	21.994163
82.941885	2610.324925	21.999181
82.909395	2608.262835	22.004199
82.690767	2610.515620	22.009216
82.857069	2605.964030	22.014234
82.978051	2598.247684	22.019251
82.982967	2603.426022	22.024269
82.901145	2614.339755	22.029287
83.049170	2608.307674	22.034304
82.605735	2605.463749	22.039322
83.241489	2618.658036	22.044339
83.471961	2628.080848	22.049357
83.415023	2642.860026	22.054375
83.548057	2633.475400	22.059392
83.485796	2633.901745	22.064410
83.442648	2634.350362	22.069427
83.472645	2627.402463	22.074445
83.405340	2649.240160	22.079463
83.662201	2655.458653	22.084480
83.801114	2654.831119	22.089498
83.966560	2656.266661	22.094515
84.210128	2667.489554	22.099533
84.335380	2677.304343	22.104551
84.284905	2671.038038	22.109568
84.890143	2666.427561	22.114586
84.552854	2677.999692	22.119603
84.692314	2678.628178	22.124621
84.547049	2670.268393	22.129639
84.731274	2672.824565	22.134656
85.041727	2675.499950	22.139674
85.319111	2679.139923	22.144691
85.533873	2685.582747	22.149709
85.226484	2676.456033	22.154727
85.517145	2681.536251	22.159744
85.794068	2685.031119	22.164762
86.198090	2683.910993	22.169779
85.750188	2665.625223	22.174797
85.742400	2661.381612	22.179815
85.526866	2654.875903	22.184832
85.655277	2669.272769	22.189850
85.693519	2680.877960	22.194867
85.970496	2688.112734	22.199885
85.985265	2690.038834	22.204903
86.024177	2682.568778	22.209920
86.179146	2678.893158	22.214938
86.071043	2686.595017	22.219955
86.231230	2695.135645	22.224973
86.437907	2701.724913	22.229991
86.299607	2698.877650	22.235008
86.344703	2704.895582	22.240026
86.592521	2708.694810	22.245043
86.780614	2718.048522	22.250061
86.455543	2728.896048	22.255079
86.754772	2726.460380	22.260096
87.062203	2725.781358	22.265114
86.731881	2730.251318	22.270131
87.237381	2736.232295	22.275149
87.365178	2749.508921	22.280167
87.313637	2752.423729	22.285184
87.583660	2743.655242	22.290202
87.477939	2750.223732	22.295219
87.960811	2749.539487	22.300237
88.120510	2747.520048	22.305255
87.850955	2744.772115	22.310272
87.808731	2743.156529	22.315290
87.671087	2757.585421	22.320307
87.954049	2751.573311	22.325325
88.205661	2759.541113	22.330343
88.392737	2762.813280	22.335360
88.391619	2766.597625	22.340378
88.384668	2765.806590	22.345395
88.394435	2759.360448	22.350413
88.462410	2759.794923	22.355431
88.706261	2780.508118	22.360448
88.816156	2778.733135	22.365466
88.611048	2781.712887	22.370483
88.935330	2780.459991	22.375501
89.439386	2778.872969	22.380519
89.062886	2775.040215	22.385536
89.289548	2769.447154	22.390554
89.012177	2772.498120	22.395571
89.443435	2787.223500	22.400589
89.267914	2788.939377	22.405607
89.671126	2790.094894	22.410624
89.963653	2793.379053	22.415642
89.979805	2794.676892	22.420659
90.219426	2802.485621	22.425677
90.368968	2786.164466	22.430695
90.334988	2793.488726	22.435712
90.708161	2791.903143	22.440730
90.161888	2794.257460	22.445747
90.277283	2793.450531	22.450765
90.770219	2794.235444	22.455783
90.603747	2797.294397	22.460800
90.884391	2791.440438	22.465818
90.501876	2792.367966	22.470835
90.651443	2801.853962	22.475853
90.975415	2789.690592	22.480871
91.027838	2811.187927	22.485888
91.396438	2815.331321	22.490906
91.082441	2817.905119	22.495923
91.235146	2814.706391	22.500941
91.242321	2816.649467	22.505959
91.155599	2821.116239	22.510976
91.476590	2815.985043	22.515994
91.311362	2826.599440	22.521011
91.630708	2833.732995	22.526029
91.741215	2842.060503	22.531047
91.835016	2848.115086	22.536064
91.889354	2838.859380	22.541082
91.475864	2845.318019	22.546099
91.880840	2858.554727	22.551117
92.121096	2863.816429	22.556135
92.218501	2872.278547	22.561152
92.175901	2864.789545	22.566170
92.652516	2865.958888	22.571187
92.282620	2868.781258	22.576205
92.798526	2882.401534	22.581223
92.926970	2884.133216	22.586240
93.305446	2891.184998	22.591258
93.195470	2892.795996	22.596275
93.176297	2894.440199	22.601293
93.099377	2881.865771	22.606311
93.246853	2890.408471	22.611328
93.592178	2888.117098	22.616346
93.076024	2886.202869	22.621363
92.921261	2893.621722	22.626381
93.549988	2904.699583	22.631399
93.601506	2916.681589	22.636416
93.760930	2915.435416	22.641434
93.779195	2914.002918	22.646451
93.669737	2915.860013	22.651469
93.993081	2931.246156	22.656487
94.041379	2938.983737	22.661504
94.489028	2942.963361	22.666522
94.592602	2936.098570	22.671539
94.330491	2942.164412	22.676557
94.552184	2926.005482	22.681575
94.653785	2933.558021	22.686592
94.898404	2922.622012	22.691610
94.685824	2943.097162	22.696627
94.801527	2948.943222	22.701645
95.104743	2957.363868	22.706663
95.202683	2955.142563	22.711680
95.354602	2950.744618	22.716698
95.090815	2956.741292	22.721715
95.283556	2954.252740	22.726733
95.714960	2948.201673	22.731751
95.508842	2943.783727	22.736768
95.573333	2955.252453	22.741786
95.975643	2968.069896	22.746803
96.096689	2973.918289	22.751821
96.467308	2963.145691	22.756839
96.157945	2972.463367	22.761856
96.093620	2976.579519	22.766874
96.406292	2976.136380	22.771891
96.119386	2968.959952	22.776909
96.010496	2963.908268	22.781927
96.016522	2971.781845	22.786944
96.242110	2988.224769	22.791962
96.497549	2988.775244	22.796979
96.837004	2989.473599	22.801997
96.692726	2985.743513	22.807015
97.060566	2999.765664	22.812032
97.041935	3004.597455	22.817050
97.442107	3013.362828	22.822067
97.221412	3018.649002	22.827085
97.665394	3013.949924	22.832103
97.454122	3011.072943	22.837120
97.121764	3016.158731	22.842138
97.612978	3022.347176	22.847155
97.749606	3038.062311	22.852173
97.889985	3029.822002	22.857191
98.076965	3034.160998	22.862208
98.065653	3037.602972	22.867226
98.462488	3035.739103	22.872243
97.911429	3043.345962	22.877261
98.378377	3048.919597	22.882279
98.266077	3062.224367	22.887296
98.448297	3060.911513	22.892314
98.535718	3054.301681	22.897331
98.670582	3063.502899	22.902349
99.104502	3069.103775	22.907367
99.184146	3078.263100	22.912384
99.200483	3071.500211	22.917402
99.296729	3073.098055	22.922419
99.074923	3078.892554	22.927437
99.012983	3073.110779	22.932455
98.876921	3086.283554	22.937472
99.426778	3093.157239	22.942490
99.811634	3107.561872	22.947507
100.221313	3107.157280	22.952525
100.512429	3100.686148	22.957543
100.129363	3090.924000	22.962560
100.317303	3096.765174	22.967578
100.259068	3098.317637	22.972595
100.424519	3097.635458	22.977613
100.602987	3089.297665	22.982631
100.548681	3093.462782	22.987648
100.673420	3093.639095	22.992666
100.771990	3089.524004	22.997683
101.105290	3105.110737	23.002701
101.454509	3104.674530	23.007719
100.699942	3097.649765	23.012736
100.896163	3107.444271	23.017754
101.340710	3119.797610	23.022771
101.044327	3106.556534	23.027789
101.409217	3110.467022	23.032807
101.533743	3109.361982	23.037824
101.469523	3113.907382	23.042842
101.536078	3113.344752	23.047859
101.339818	3128.092367	23.052877
101.530329	3129.435674	23.057895
101.807312	3132.002719	23.062912
101.661062	3133.493142	23.067930
102.318404	3141.678840	23.072947
102.117553	3169.881779	23.077965
102.778712	3166.376585	23.082983
102.947359	3167.000545	23.088000
102.441269	3169.698983	23.093018
102.453456	3159.909977	23.098035
102.465004	3172.980930	23.103053
102.643575	3163.800399	23.108071
102.921849	3180.885459	23.113088
103.010037	3189.415440	23.118106
103.320383	3182.745604	23.123123
103.125545	3192.509514	23.128141
103.047016	3183.144917	23.133159
103.498316	3191.189130	23.138176
103.228705	3201.974651	23.143194
103.666458	3203.134287	23.148211
103.485252	3209.780976	23.153229
103.770322	3205.583168	23.158247
103.743342	3215.358830	23.163264
103.968021	3221.244823	23.168282
104.088202	3227.121838	23.173299
104.195267	3229.955219	23.178317
104.429850	3223.300320	23.183335
104.541200	3227.821570	23.188352
104.614873	3242.943863	23.193370
105.273481	3256.311808	23.198387
105.411052	3251.133299	23.203405
105.678284	3244.577461	23.208423
105.423375	3244.970691	23.213440
105.565340	3237.844161	23.218458
105.688140	3241.265293	23.223475
105.328542	3245.878807	23.228493
105.249086	3242.640403	23.233511
105.204834	3241.012463	23.238528
105.134423	3248.105870	23.243546
105.462082	3251.056404	23.248563
106.176364	3256.089769	23.253581
105.969029	3262.418619	23.258599
106.079528	3272.917758	23.263616
106.112850	3278.558978	23.268634
106.296956	3272.205442	23.273651
106.272089	3288.012218	23.278669
106.541948	3292.660301	23.283687
106.461746	3288.134293	23.288704
106.708434	3295.314063	23.293722
106.769498	3291.419384	23.298739
106.854296	3303.099788	23.303757
107.008219	3309.028388	23.308775
107.362496	3310.680764	23.313792
107.162610	3305.740993	23.318810
107.572359	3303.729903	23.323827
107.570381	3309.449220	23.328845
107.542165	3314.857008	23.333863
107.716973	3332.018289	23.338880
107.677801	3331.768792	23.343898
107.997114	3317.866748	23.348915
108.218465	3325.075724	23.353933
108.469878	3321.741604	23.358951
108.525829	3318.242236	23.363968
108.471583	3324.206407	23.368986
108.961504	3313.165690	23.374003
108.636806	3318.704855	23.379021
108.873950	3314.845880	23.384039
108.739142	3312.247312	23.389056
108.954917	3315.862290	23.394074
109.216266	3327.493129	23.399091
109.212747	3341.851108	23.404109
109.151478	3341.557709	23.409127
109.311396	3338.493481	23.414144
109.143839	3339.201353	23.419162
109.779353	3344.294350	23.424179
109.814758	3339.573585	23.429197
109.525468	3334.988590	23.434215
110.004334	3337.940847	23.439232
110.001483	3350.319815	23.444250
110.042313	3349.066827	23.449267
110.014105	3349.330079	23.454285
110.514674	3357.177326	23.459303
109.975852	3358.406959	23.464320
109.856900	3354.442453	23.469338
109.965609	3364.465344	23.474355
110.102058	3373.720129	23.479373
110.507618	3394.418325	23.484391
110.810566	3400.860302	23.489408
110.433382	3403.440863	23.494426
110.854866	3418.152503	23.499443
111.075569	3427.520445	23.504461
111.260083	3433.823065	23.509479
111.375492	3434.508978	23.514496
111.639178	3449.166308	23.519514
111.833253	3457.935581	23.524531
112.045784	3460.140279	23.529549
112.174424	3452.744306	23.534567
112.600086	3448.849640	23.539584
112.364593	3453.134578	23.544602
112.678770	3437.765617	23.549619
112.897884	3445.186453	23.554637
112.677033	3455.235456	23.559655
112.932475	3451.976433	23.564672
112.714786	3450.574317	23.569690
112.851681	3450.177472	23.574707
113.009081	3455.575341	23.579725
113.064317	3472.742747	23.584743
113.292554	3473.673059	23.589760
113.287174	3482.561771	23.594778
113.133856	3479.148608	23.599795
113.168267	3488.599241	23.604813
113.358792	3498.271757	23.609831
113.532172	3497.143306	23.614848
113.533967	3503.221903	23.619866
114.402640	3509.424343	23.624883
114.151351	3520.292418	23.629901
114.077187	3521.209846	23.634919
114.273109	3519.664423	23.639936
114.067454	3523.042062	23.644954
114.337537	3532.818988	23.649971
114.548546	3538.502061	23.654989
114.888112	3534.980587	23.660007
115.487718	3539.905640	23.665024
114.730607	3545.335451	23.670042
115.087478	3541.612441	23.675059
115.318543	3552.705275	23.680077
115.407588	3557.182737	23.685095
115.323665	3562.015376	23.690112
115.294790	3567.028817	23.695130
115.517848	3564.216685	23.700147
115.474948	3573.130220	23.705165
115.404812	3583.301014	23.710183
115.824521	3584.700201	23.715200
116.191676	3587.770891	23.720218
116.156321	3591.854267	23.725235
116.426396	3595.883779	23.730253
116.657521	3609.851944	23.735271
117.031918	3610.623790	23.740288
116.791253	3613.915366	23.745306
116.928885	3603.074507	23.750323
117.418484	3612.810987	23.755341
116.914399	3611.207264	23.760359
116.996976	3612.592662	23.765376
117.248450	3625.617120	23.770394
117.173734	3627.206913	23.775411
117.417312	3622.040200	23.780429
117.318474	3626.780491	23.785447
117.771834	3637.400054	23.790464
117.227652	3653.796155	23.795482
117.966948	3654.198726	23.800499
118.085142	3659.795289	23.805517
118.247362	3662.613839	23.810535
118.543200	3666.844510	23.815552
118.435585	3686.786541	23.820570
118.433528	3679.410825	23.825587
118.706631	3680.170039	23.830605
118.281200	3687.101113	23.835623
118.731435	3691.364563	23.840640
119.489862	3696.261775	23.845658
119.017645	3697.380060	23.850675
119.590432	3700.614440	23.855693
119.404551	3699.481943	23.860711
120.001792	3698.265395	23.865728
119.676985	3709.542714	23.870746
120.443991	3717.165577	23.875763
120.056055	3720.909348	23.880781
120.088397	3719.966967	23.885799
120.304218	3713.472621	23.890816
120.078458	3713.233232	23.895834
120.406096	3722.262744	23.900851
120.630202	3727.836525	23.905869
120.499926	3743.300302	23.910887
121.003336	3736.331924	23.915904
121.006121	3737.439382	23.920922
120.747784	3741.869976	23.925939
121.285316	3751.722162	23.930957
121.628267	3753.423688	23.935975
122.088716	3765.273154	23.940992
121.911170	3765.420788	23.946010
121.822936	3756.000591	23.951027
121.681951	3766.378205	23.956045
121.555294	3766.480040	23.961063
121.781126	3767.110900	23.966080
122.172563	3773.362485	23.971098
122.166775	3783.065718	23.976115
122.430819	3787.206680	23.981133
122.332833	3794.083657	23.986151
122.288500	3785.344671	23.991168
122.720717	3792.322161	23.996186
123.078448	3800.374904	24.001203
123.134239	3796.777624	24.006221
123.103745	3811.010770	24.011239
123.388345	3810.376297	24.016256
123.444827	3821.427040	24.021274
123.601127	3808.951372	24.026291
123.689344	3811.030281	24.031309
123.753672	3821.991429	24.036327
123.840394	3823.855948	24.041344
123.750945	3826.909394	24.046362
123.981168	3834.363380	24.051379
124.395761	3824.874330	24.056397
124.150482	3825.408103	24.061415
124.482491	3829.128181	24.066432
124.270262	3847.981992	24.071450
124.799445	3851.684001	24.076467
124.878866	3845.709532	24.081485
124.867218	3861.577878	24.086503
124.845998	3845.080351	24.091520
124.829996	3861.107187	24.096538
124.844174	3871.274484	24.101555
125.598032	3869.970416	24.106573
125.407141	3869.870784	24.111591
125.170512	3874.900875	24.116608
125.241327	3882.505950	24.121626
125.649754	3896.683452	24.126643
125.767167	3897.867760	24.131661
125.926270	3919.756967	24.136679
126.222590	3923.261683	24.141696
126.366098	3927.610820	24.146714
126.167247	3930.605567	24.151731
127.017690	3937.691594	24.156749
127.104120	3946.768241	24.161767
127.003864	3940.013710	24.166784
127.230404	3946.934907	24.171802
126.990620	3957.416388	24.176819
127.315545	3946.887041	24.181837
127.224038	3953.412724	24.186855
127.886049	3958.637491	24.191872
127.643064	3965.259357	24.196890
127.655038	3968.293880	24.201907
128.185817	3968.394360	24.206925
127.728159	3974.762431	24.211943
128.351176	3986.163793	24.216960
128.299193	3991.010510	24.221978
128.444642	3994.475604	24.226995
129.122794	3991.365300	24.232013
128.752926	3993.774366	24.237031
128.786189	3990.780247	24.242048
129.337329	4013.643790	24.247066
129.042503	4010.451403	24.252083
129.285592	4005.439314	24.257101
129.272047	4011.848723	24.262119
129.668953	4012.749647	24.267136
130.064744	4013.319336	24.272154
129.890927	4031.854886	24.277171
130.180094	4030.228621	24.282189
129.870560	4036.359025	24.287207
130.174307	4030.150723	24.292224
130.326741	4026.487851	24.297242
130.437597	4030.318154	24.302259
130.650901	4040.634452	24.307277
130.698126	4052.463224	24.312295
130.944241	4047.602155	24.317312
131.120178	4049.512777	24.322330
131.147929	4056.259807	24.327347
131.156551	4046.335154	24.332365
131.605158	4059.685895	24.337383
131.366773	4062.443784	24.342400
131.469223	4074.109314	24.347418
131.734963	4078.303737	24.352435
131.330551	4064.510642	24.357453
131.387333	4087.362869	24.362471
131.692384	4087.956156	24.367488
131.914961	4097.043245	24.372506
132.145784	4119.136156	24.377523
132.588545	4115.330219	24.382541
132.485325	4132.664956	24.387559
132.220823	4132.081244	24.392576
132.596547	4136.245931	24.397594
132.654066	4151.639786	24.402611
132.934329	4151.372108	24.407629
133.057657	4169.801566	24.412647
133.168805	4176.257903	24.417664
133.734873	4173.780499	24.422682
133.629940	4177.868528	24.427699
133.574759	4169.443519	24.432717
133.773095	4186.194786	24.437735
134.214556	4185.851509	24.442752
134.884830	4182.934935	24.447770
134.697793	4178.529495	24.452787
134.831837	4176.384483	24.457805
134.591697	4178.795469	24.462823
135.156331	4177.056865	24.467840
135.389545	4174.924821	24.472858
135.187156	4180.060136	24.477875
135.148026	4179.289830	24.482893
135.061507	4191.006951	24.487911
135.381677	4192.794130	24.492928
135.685315	4202.209533	24.497946
135.646121	4204.131572	24.502963
135.934234	4198.430656	24.507981
136.046375	4214.232694	24.512999
136.166687	4221.814425	24.518016
136.394479	4217.063477	24.523034
136.344556	4221.846810	24.528051
136.681827	4218.076213	24.533069
136.375922	4226.333473	24.538087
136.348058	4240.648612	24.543104
136.311215	4246.843946	24.548122
136.483566	4256.791142	24.553139
136.737824	4274.985693	24.558157
136.782504	4282.718102	24.563175
136.844591	4296.245980	24.568192
137.405766	4301.865308	24.573210
137.062734	4308.067301	24.578227
137.254388	4324.510416	24.583245
137.764630	4342.226450	24.588263
138.298626	4351.552408	24.593280
138.416353	4360.245630	24.598298
138.313736	4359.482045	24.603315
138.718566	4352.696067	24.608333
138.692566	4367.771694	24.613351
138.750781	4375.577788	24.618368
139.110614	4373.290284	24.623386
139.183000	4378.404969	24.628403
139.167604	4389.157929	24.633421
139.483577	4389.307639	24.638439
139.294270	4392.209441	24.643456
139.899577	4401.918866	24.648474
139.781879	4403.528044	24.653491
140.010575	4402.962226	24.658509
140.054330	4416.392045	24.663527
140.203353	4422.558501	24.668544
140.565783	4421.495251	24.673562
140.847477	4425.441076	24.678579
140.826675	4425.845225	24.683597
141.213301	4435.172077	24.688615
141.001481	4439.065330	24.693632
141.566061	4434.265048	24.698650
140.945104	4441.630863	24.703667
141.452455	4446.125485	24.708685
141.187663	4438.402132	24.713703
141.373790	4462.058503	24.718720
141.779622	4470.381818	24.723738
141.742562	4464.185396	24.728755
141.903202	4472.982464	24.733773
142.031741	4475.446561	24.738791
142.069119	4488.593354	24.743808
142.765173	4487.610725	24.748826
142.359867	4495.009270	24.753843
142.543065	4495.883522	24.758861
142.749471	4505.705611	24.763879
143.600240	4491.126528	24.768896
144.070998	4497.429143	24.773914
144.213728	4489.683354	24.778931
143.803277	4484.280492	24.783949
144.192361	4481.006792	24.788967
144.565043	4481.469623	24.793984
144.751238	4487.898604	24.799002
144.812830	4482.971457	24.804019
144.255714	4468.867252	24.809037
144.746002	4461.121021	24.814055
144.769495	4477.243257	24.819072
145.052934	4465.315488	24.824090
145.075509	4477.501888	24.829107
144.878565	4481.989387	24.834125
145.092158	4477.654066	24.839143
144.730512	4478.306977	24.844160
145.141817	4491.300864	24.849178
145.299964	4496.755744	24.854195
145.352684	4505.938924	24.859213
145.518349	4516.234505	24.864231
145.789747	4531.169274	24.869248
146.039896	4519.133023	24.874266
146.460611	4529.559346	24.879283
146.130788	4542.870665	24.884301
146.976091	4552.504931	24.889319
146.368487	4559.635142	24.894336
146.839598	4548.571354	24.899354
146.835218	4565.720673	24.904371
146.555452	4575.959382	24.909389
146.887542	4585.367400	24.914407
146.951215	4602.783920	24.919424
147.067345	4609.981386	24.924442
147.233500	4616.950119	24.929459
147.461893	4633.681339	24.934477
147.816523	4635.419009	24.939495
148.071697	4655.447662	24.944512
148.077140	4661.500829	24.949530
148.257816	4666.362006	24.954547
148.081140	4679.469667	24.959565
148.747322	4678.636875	24.964583
148.496353	4693.264870	24.969600
148.749964	4704.664229	24.974618
149.037075	4716.184637	24.979635
148.962576	4722.445968	24.984653
149.512069	4723.499932	24.989671
149.692352	4744.755559	24.994688
149.886937	4738.901747	24.999706
149.887126	4732.592117	25.004723
150.070534	4741.183760	25.009741
150.604256	4756.257790	25.014759
150.281670	4762.990187	25.019776
150.663703	4761.876521	25.024794
150.623588	4766.702659	25.029811
150.953030	4777.357972	25.034829
151.310630	4779.155165	25.039847
151.395965	4791.941193	25.044864
151.463412	4792.836638	25.049882
151.379021	4794.083989	25.054899
151.009924	4797.430494	25.059917
151.699830	4799.403214	25.064935
151.792434	4803.211272	25.069952
152.011115	4806.030680	25.074970
151.696666	4804.820281	25.079987
152.011580	4830.000570	25.085005
152.380342	4824.012294	25.090023
152.256562	4834.779237	25.095040
152.616166	4847.109111	25.100058
153.029259	4851.217645	25.105075
153.146479	4860.302583	25.110093
153.423154	4845.253911	25.115111
153.441917	4853.097918	25.120128
153.931242	4863.570567	25.125146
153.873795	4873.774830	25.130163
153.759601	4873.704283	25.135181
154.079364	4866.107531	25.140199
154.093458	4875.593617	25.145216
154.049280	4880.635056	25.150234
154.906446	4884.144178	25.155251
154.559459	4893.490792	25.160269
154.960888	4893.362062	25.165287
154.958377	4892.024179	25.170304
154.969041	4899.818964	25.175322
155.004636	4908.414761	25.180339
155.409702	4908.923065	25.185357
155.907911	4909.975556	25.190375
155.816816	4923.130041	25.195392
155.795771	4939.834094	25.200410
156.158219	4933.022935	25.205427
155.769793	4942.303428	25.210445
156.169263	4942.462238	25.215463
156.803498	4955.131359	25.220480
156.532396	4964.261025	25.225498
156.536390	4964.446687	25.230515
156.804557	4973.691255	25.235533
157.064257	4985.976806	25.240551
157.015134	4991.928103	25.245568
156.830186	4995.271225	25.250586
157.546720	5011.794224	25.255603
157.501779	5018.360387	25.260621
157.962100	5023.159184	25.265639
157.839662	5036.580616	25.270656
158.320605	5030.492740	25.275674
158.375134	5033.501878	25.280691
158.229652	5038.925281	25.285709
158.904684	5044.833293	25.290727
158.964442	5058.333695	25.295744
158.841630	5060.956951	25.300762
159.207519	5070.359959	25.305779
159.522356	5080.970377	25.310797
160.068984	5071.996721	25.315815
160.043665	5075.659059	25.320832
160.100125	5079.081400	25.325850
160.171510	5075.740270	25.330867
159.970325	5089.530682	25.335885
160.153172	5102.046073	25.340903
160.469946	5094.036194	25.345920
160.517273	5112.730962	25.350938
161.171985	5130.008622	25.355955
160.744482	5128.923122	25.360973
160.934537	5128.303325	25.365991
160.949984	5139.146622	25.371008
161.236643	5148.830307	25.376026
161.612705	5157.351119	25.381043
161.554435	5173.685562	25.386061
161.928662	5178.822922	25.391079
161.978152	5180.794385	25.396096
162.032463	5182.528362	25.401114
162.561733	5189.260863	25.406131
162.707618	5202.593295	25.411149
163.101021	5196.531619	25.416167
163.315183	5194.733854	25.421184
162.942928	5199.220415	25.426202
162.868046	5191.700753	25.431219
163.011108	5212.817525	25.436237
163.017156	5209.110920	25.441255
163.617036	5228.543623	25.446272
164.291861	5234.476982	25.451290
164.805106	5236.073226	25.456307
164.532010	5239.761548	25.461325
164.675705	5236.314435	25.466343
164.769298	5239.011345	25.471360
164.672548	5241.450649	25.476378
165.030267	5240.280767	25.481395
165.074720	5237.363614	25.486413
165.286333	5228.483074	25.491431
165.499021	5258.070554	25.496448
165.315886	5263.755563	25.501466
165.511525	5259.034603	25.506483
165.518999	5268.509299	25.511501
165.856801	5277.676894	25.516519
165.739479	5285.558057	25.521536
166.031424	5293.448103	25.526554
166.632608	5308.366891	25.531571
166.271710	5306.800690	25.536589
166.195120	5313.810641	25.541607
166.695067	5326.835520	25.546624
166.793626	5330.933160	25.551642
167.283046	5341.712254	25.556659
167.210588	5352.856607	25.561677
167.493838	5358.475346	25.566695
167.434686	5370.798175	25.571712
167.595219	5371.944302	25.576730
168.150755	5385.819141	25.581747
168.154272	5403.207917	25.586765
168.269579	5399.891454	25.591783
168.622800	5402.601628	25.596800
168.997745	5428.991819	25.601818
169.225384	5422.485555	25.606835
169.191313	5437.449691	25.611853
169.395477	5428.084109	25.616871
169.348945	5455.142855	25.621888
169.553730	5463.561061	25.626906
169.640948	5455.283737	25.631923
170.289048	5471.953543	25.636941
169.878187	5486.925878	25.641959
169.931447	5491.835524	25.646976
170.080781	5514.744583	25.651994
170.486294	5515.063444	25.657011
170.489880	5525.473215	25.662029
171.009530	5538.665632	25.667047
171.207375	5538.735893	25.672064
171.323834	5545.517015	25.677082
171.939906	5553.142066	25.682100
171.815445	5556.267541	25.687117
171.885844	5556.190347	25.692135
171.947305	5557.099387	25.697152
172.227683	5575.316430	25.702170
172.623819	5572.593837	25.707188
172.535557	5574.511033	25.712205
172.867234	5596.167064	25.717223
173.417413	5597.697617	25.722240
173.629634	5603.652616	25.727258
173.830041	5599.887263	25.732276
173.637448	5596.252541	25.737293
173.446006	5594.593644	25.742311
173.972623	5608.618358	25.747328
174.065185	5616.593249	25.752346
174.467677	5615.703620	25.757364
174.529840	5615.637178	25.762381
174.723596	5621.756043	25.767399
174.866424	5616.209882	25.772416
175.063005	5619.455838	25.777434
174.983865	5633.483341	25.782452
175.164551	5639.446419	25.787469
175.249925	5636.999472	25.792487
175.504799	5633.547601	25.797504
175.980400	5648.921827	25.802522
175.986150	5658.425404	25.807540
176.201809	5658.581276	25.812557
176.395344	5662.149683	25.817575
176.517496	5660.546123	25.822592
176.247709	5666.134268	25.827610
176.681620	5679.592662	25.832628
176.780546	5679.971885	25.837645
176.990835	5686.378603	25.842663
176.767097	5702.057462	25.847680
177.091904	5722.076451	25.852698
177.464392	5718.568375	25.857716
177.623017	5730.816505	25.862733
178.035303	5740.711378	25.867751
178.302989	5742.427971	25.872768
178.073688	5759.395630	25.877786
178.293211	5769.143761	25.882804
178.115322	5776.712594	25.887821
178.825760	5783.997923	25.892839
178.880935	5794.062060	25.897856
179.003000	5799.264110	25.902874
179.331866	5819.083709	25.907892
179.410688	5824.399822	25.912909
179.288037	5837.149522	25.917927
179.425912	5840.660342	25.922944
179.646522	5865.127575	25.927962
180.197693	5869.631517	25.932980
180.427604	5875.498623	25.937997
180.866344	5888.296690	25.943015
181.257881	5887.752825	25.948032
181.119570	5898.042853	25.953050
181.275420	5897.889222	25.958068
181.979967	5904.793568	25.963085
181.754835	5918.758791	25.968103
181.967668	5921.159457	25.973120
182.109548	5915.809062	25.978138
182.292041	5924.584492	25.983156
182.475098	5937.365582	25.988173
182.233321	5937.797855	25.993191
182.625253	5930.697641	25.998208
182.475334	5953.297146	26.003226
183.106003	5958.098081	26.008244
183.328155	5961.958815	26.013261
183.624708	5980.356829	26.018279
184.026414	5985.569057	26.023296
183.767094	5988.800830	26.028314
183.914441	5999.030658	26.033332
184.116690	6009.775944	26.038349
184.218541	6017.569637	26.043367
184.342323	6008.866538	26.048384
184.061212	6033.232181	26.053402
184.676045	6040.425174	26.058420
185.102346	6053.534644	26.063437
185.155558	6063.040511	26.068455
184.975680	6071.367368	26.073472
185.288635	6089.036912	26.078490
185.780979	6083.590868	26.083508
186.215483	6101.465621	26.088525
186.250187	6108.007150	26.093543
186.477126	6102.943339	26.098560
186.680141	6117.504951	26.103578
186.699437	6113.174241	26.108596
187.112847	6121.714946	26.113613
187.285992	6132.307004	26.118631
187.428824	6137.891028	26.123648
187.464831	6145.676087	26.128666
187.525077	6129.997156	26.133684
187.380226	6137.750393	26.138701
187.601362	6152.205042	26.143719
188.038424	6156.420626	26.148736
187.987974	6171.425795	26.153754
188.140968	6182.554493	26.158772
188.991931	6184.240295	26.163789
188.823311	6201.258893	26.168807
189.260697	6202.267272	26.173824
189.645245	6207.611658	26.178842
189.747350	6217.040547	26.183860
190.238107	6221.632900	26.188877
190.116262	6222.068603	26.193895
190.181508	6213.923780	26.198912
190.406434	6230.426575	26.203930
190.613497	6242.673821	26.208948
190.522060	6244.294854	26.213965
190.595302	6252.869642	26.218983
191.286154	6265.641350	26.224000
190.845900	6266.186605	26.229018
191.052255	6282.417707	26.234036
191.449340	6291.131495	26.239053
191.473027	6304.742606	26.244071
191.859627	6307.703411	26.249088
192.137054	6316.274850	26.254106
192.041222	6329.036500	26.259124
192.377510	6331.919912	26.264141
192.567314	6347.048810	26.269159
192.850329	6356.847348	26.274176
193.039282	6373.677855	26.279194
193.150841	6378.313501	26.284212
193.451483	6390.063304	26.289229
193.503448	6407.199272	26.294247
193.732517	6419.272749	26.299264
194.239961	6431.347089	26.304282
194.478200	6434.703503	26.309300
195.005263	6440.044711	26.314317
194.913444	6458.462636	26.319335
194.600020	6452.920965	26.324352
195.182072	6460.747413	26.329370
195.466797	6472.906962	26.334388
195.867409	6472.873055	26.339405
195.863964	6486.444332	26.344423
196.191530	6487.327773	26.349440
196.018518	6501.146431	26.354458
195.932357	6507.817405	26.359476
196.593050	6521.935592	26.364493
196.466918	6533.928708	26.369511
196.864802	6534.867495	26.374528
197.015127	6547.714086	26.379546
197.406878	6556.643488	26.384564
197.662465	6554.390888	26.389581
197.895876	6565.488360	26.394599
198.236899	6584.151538	26.399616
197.870328	6588.463930	26.404634
197.991025	6596.425399	26.409652
198.950943	6596.026623	26.414669
198.948416	6601.775473	26.419687
199.035486	6595.315932	26.424704
199.468083	6610.224157	26.429722
198.999912	6618.031092	26.434740
199.604035	6626.858016	26.439757
199.548100	6626.099692	26.444775
199.783559	6629.257702	26.449792
200.169207	6639.501296	26.454810
199.879557	6653.316130	26.459828
200.112335	6654.994052	26.464845
200.519321	6672.166540	26.469863
200.869535	6680.370106	26.474880
200.971668	6695.102566	26.479898
201.043192	6703.059110	26.484916
201.427468	6701.297850	26.489933
201.415154	6707.161900	26.494951
201.984067	6721.423958	26.499968
202.219902	6721.055836	26.504986
202.134225	6729.320974	26.510004
202.107727	6738.536555	26.515021
202.170854	6747.892867	26.520039
202.449156	6760.946970	26.525056
202.939628	6767.244155	26.530074
202.971852	6787.732872	26.535092
203.138151	6788.953956	26.540109
203.297278	6799.176085	26.545127
203.650605	6813.777986	26.550144
203.793932	6818.822334	26.555162
204.338722	6836.870045	26.560180
204.470768	6853.788773	26.565197
204.453211	6870.137334	26.570215
204.768517	6874.832932	26.575232
204.930867	6882.245076	26.580250
204.904140	6893.200154	26.585268
205.284897	6894.858216	26.590285
205.614323	6916.430933	26.595303
205.957281	6926.337246	26.600320
206.356846	6919.462751	26.605338
206.182939	6930.560724	26.610356
206.632582	6946.265238	26.615373
206.703077	6957.138925	26.620391
207.101006	6955.463906	26.625408
207.175845	6979.033543	26.630426
207.499818	6986.502643	26.635444
207.885824	6987.935764	26.640461
207.728707	7004.154647	26.645479
207.855038	7011.765015	26.650496
208.247199	7014.362039	26.655514
208.640611	7027.073260	26.660532
209.076657	7027.431595	26.665549
208.921643	7033.668371	26.670567
208.861358	7045.882016	26.675584
209.487664	7050.390340	26.680602
209.300718	7057.626490	26.685620
209.746081	7064.798923	26.690637
209.981178	7077.471691	26.695655
209.846096	7080.835838	26.700672
210.563375	7101.192996	26.705690
210.230559	7108.082528	26.710708
210.685889	7113.927566	26.715725
211.030714	7119.688793	26.720743
211.147615	7110.885224	26.725760
211.583431	7127.109764	26.730778
211.570333	7147.583842	26.735796
212.040988	7143.741374	26.740813
211.835745	7155.706174	26.745831
211.978000	7181.083905	26.750848
212.832044	7163.992519	26.755866
212.703985	7176.185234	26.760884
213.004405	7177.322327	26.765901
213.305028	7185.751662	26.770919
213.480953	7188.694903	26.775936
213.776699	7202.175934	26.780954
214.040883	7210.569915	26.785972
213.867958	7223.754579	26.790989
214.050002	7215.316482	26.796007
214.360325	7221.240954	26.801024
214.437797	7232.921869	26.806042
214.634013	7235.271630	26.811060
215.207839	7240.429011	26.816077
214.873849	7247.726010	26.821095
215.117192	7254.825795	26.826112
215.155236	7269.881222	26.831130
215.359658	7288.108644	26.836148
215.542466	7299.526967	26.841165
216.136733	7315.982710	26.846183
215.907227	7328.566986	26.851200
216.456577	7341.629813	26.856218
216.487473	7359.862224	26.861236
216.569293	7372.685334	26.866253
216.877562	7376.526648	26.871271
216.862112	7400.208746	26.876288
217.401945	7413.064753	26.881306
217.726152	7435.923740	26.886324
218.189286	7437.745813	26.891341
218.362863	7457.581897	26.896359
218.115949	7469.480780	26.901376
218.859041	7480.401592	26.906394
219.097394	7490.434987	26.911412
219.197649	7479.433487	26.916429
219.888386	7503.122577	26.921447
219.759876	7518.560866	26.926464
220.460707	7513.940618	26.931482
220.192850	7520.674973	26.936500
220.404622	7528.063900	26.941517
220.907364	7520.819548	26.946535
220.952251	7530.532671	26.951552
221.262481	7542.439567	26.956570
221.421547	7547.895219	26.961588
221.787499	7557.419467	26.966605
222.205452	7576.488390	26.971623
222.020616	7584.185324	26.976640
222.323801	7572.763876	26.981658
222.439152	7596.795220	26.986676
222.795011	7602.558039	26.991693
222.868835	7602.511873	26.996711
222.975586	7633.265647	27.001728
223.365806	7635.102249	27.006746
223.361999	7648.541851	27.011764
223.475870	7652.653414	27.016781
224.023738	7661.025534	27.021799
224.301691	7684.037250	27.026816
224.322783	7688.949337	27.031834
224.505324	7699.424033	27.036852
224.469000	7709.468743	27.041869
225.084329	7711.870121	27.046887
225.212454	7734.308568	27.051904
225.426019	7735.983268	27.056922
225.488832	7758.173045	27.061940
225.518950	7766.846806	27.066957
226.075112	7780.881221	27.071975
226.144294	7796.323691	27.076992
226.856492	7805.797319	27.082010
227.283217	7816.540288	27.087028
227.149195	7812.842335	27.092045
227.694052	7827.257379	27.097063
227.522052	7836.000523	27.102080
227.836887	7838.079340	27.107098
228.345060	7861.926751	27.112116
228.457022	7860.454022	27.117133
228.942733	7868.709637	27.122151
228.558047	7866.578661	27.127168
229.203391	7884.251859	27.132186
229.061832	7896.904910	27.137204
229.012485	7892.792826	27.142221
229.376467	7910.134176	27.147239
229.489034	7923.063376	27.152256
229.665600	7930.742072	27.157274
229.593097	7941.717529	27.162292
229.899497	7955.112217	27.167309
230.282706	7969.716701	27.172327
230.062974	7994.583660	27.177344
230.800581	8006.730545	27.182362
230.845738	8027.670078	27.187380
231.180043	8044.921466	27.192397
231.938489	8052.610644	27.197415
231.988962	8066.338857	27.202432
232.163422	8076.524584	27.207450
232.425184	8082.971484	27.212468
232.822689	8103.423740	27.217485
232.947877	8095.606548	27.222503
233.095778	8116.997420	27.227520
233.575940	8123.116733	27.232538
233.751545	8132.724583	27.237556
233.816686	8148.126936	27.242573
234.523971	8148.667215	27.247591
234.302267	8167.416459	27.252608
235.081449	8174.076436	27.257626
235.210561	8181.295389	27.262644
235.163026	8192.585965	27.267661
235.583913	8197.723232	27.272679
235.408250	8211.426776	27.277696
236.390512	8228.523789	27.282714
236.138461	8229.263940	27.287732
236.699233	8236.494635	27.292749
237.180501	8245.126796	27.297767
237.051874	8257.355041	27.302784
237.116666	8246.939496	27.307802
237.434788	8266.854972	27.312820
237.731782	8275.777869	27.317837
237.885690	8281.313468	27.322855
238.289255	8313.619618	27.327872
238.250028	8307.867370	27.332890
238.365575	8322.545377	27.337908
238.777551	8333.755029	27.342925
239.167880	8332.658809	27.347943
239.231742	8350.625035	27.352960
239.420304	8353.575968	27.357978
239.245844	8365.937702	27.362996
239.784878	8376.028951	27.368013
240.432054	8395.890180	27.373031
240.353587	8418.358467	27.378048
240.367396	8417.096712	27.383066
240.612698	8431.037956	27.388084
241.008442	8447.134149	27.393101
241.488705	8451.166749	27.398119
241.579566	8478.224348	27.403136
241.739711	8492.677711	27.408154
241.719515	8504.036833	27.413172
241.882249	8523.149630	27.418189
242.275519	8537.569890	27.423207
242.592798	8549.994100	27.428224
242.645352	8565.341933	27.433242
243.159536	8583.023595	27.438260
243.062479	8604.601552	27.443277
243.549818	8613.100344	27.448295
243.608546	8631.926367	27.453312
243.632864	8640.443588	27.458330
244.122432	8657.532466	27.463348
244.316745	8675.084063	27.468365
244.925718	8689.900223	27.473383
244.902775	8703.971834	27.478400
244.806106	8718.143332	27.483418
245.530054	8730.138127	27.488436
245.541680	8739.017278	27.493453
246.223813	8749.954656	27.498471
246.807587	8764.493817	27.503488
246.554227	8777.878382	27.508506
246.818744	8783.561081	27.513524
247.210811	8801.476647	27.518541
247.414841	8797.890035	27.523559
247.079306	8816.720801	27.528576
247.779505	8823.402784	27.533594
248.143982	8838.973793	27.538612
248.345958	8857.676717	27.543629
248.318748	8863.171232	27.548647
248.774543	8878.964841	27.553664
249.016299	8891.252655	27.558682
249.488444	8900.227513	27.563700
250.048969	8904.825472	27.568717
250.370604	8908.134631	27.573735
250.644883	8923.391414	27.578752
250.783506	8913.535438	27.583770
251.215024	8933.623408	27.588788
251.290031	8942.353876	27.593805
251.445011	8948.760876	27.598823
251.560458	8955.957003	27.603840
251.844362	8971.000798	27.608858
251.836152	8978.490856	27.613876
252.398457	8989.166047	27.618893
252.450833	8997.603292	27.623911
252.636025	9015.664932	27.628928
252.649462	9023.704138	27.633946
253.426464	9031.239298	27.638964
253.255348	9048.434556	27.643981
253.783795	9058.395229	27.648999
254.081402	9075.340737	27.654016
254.187499	9088.622205	27.659034
254.521388	9096.311623	27.664052
254.749280	9117.306027	27.669069
255.273024	9126.841252	27.674087
255.244769	9139.559598	27.679104
255.560525	9143.737936	27.684122
255.818228	9141.686755	27.689140
255.836410	9165.687912	27.694157
256.760281	9171.454351	27.699175
256.582701	9185.531459	27.704192
256.613344	9207.494355	27.709210
257.090274	9214.637461	27.714228
257.163706	9227.377922	27.719245
257.636406	9234.215448	27.724263
257.945709	9246.603483	27.729280
257.884672	9255.374221	27.734298
258.692130	9260.000126	27.739316
258.815047	9273.440124	27.744333
259.142396	9276.903163	27.749351
259.562290	9291.190423	27.754368
259.761864	9302.957827	27.759386
259.872125	9299.578306	27.764404
259.940013	9320.840955	27.769421
260.363170	9321.763331	27.774439
260.384318	9346.676690	27.779456
260.658412	9361.690759	27.784474
261.147292	9372.974315	27.789492
260.961585	9386.613990	27.794509
261.509665	9392.855756	27.799527
261.395954	9404.308920	27.804544
261.444180	9417.416515	27.809562
262.184110	9430.725837	27.814580
262.459573	9442.150007	27.819597
262.407751	9461.363479	27.824615
262.991809	9467.950121	27.829632
262.839760	9491.911901	27.834650
263.299756	9495.310128	27.839668
263.033912	9525.490457	27.844685
263.642498	9536.711276	27.849703
264.461237	9548.341395	27.854720
264.398106	9563.648079	27.859738
264.778511	9572.880656	27.864756
264.759987	9590.731466	27.869773
265.030246	9602.304935	27.874791
265.550306	9611.566305	27.879808
265.344191	9632.862498	27.884826
265.817858	9648.928665	27.889844
266.162093	9663.133274	27.894861
266.479732	9678.339726	27.899879
266.505947	9685.209045	27.904896
266.922940	9705.972611	27.909914
267.488905	9719.899634	27.914932
267.697616	9741.857539	27.919949
268.008273	9748.149020	27.924967
268.083209	9767.302028	27.929984
268.455911	9785.111059	27.935002
268.782215	9787.488255	27.940020
268.835038	9813.650746	27.945037
269.113884	9824.746269	27.950055
269.892706	9838.403446	27.955072
269.933662	9857.713387	27.960090
270.264524	9858.467039	27.965108
270.731424	9870.338419	27.970125
271.223722	9883.607689	27.975143
271.406357	9895.482297	27.980160
271.604980	9905.971528	27.985178
271.997262	9902.386970	27.990196
272.341826	9921.943339	27.995213
272.299488	9918.546419	28.000231
272.552734	9934.224072	28.005248
272.535415	9953.941006	28.010266
272.887370	9959.361028	28.015284
273.416062	9977.281722	28.020301
273.586201	9998.327160	28.025319
274.036106	10002.923674	28.030336
273.962218	10023.268321	28.035354
274.327921	10023.441924	28.040372
275.025052	10032.827489	28.045389
275.166883	10056.589534	28.050407
275.377727	10053.765693	28.055424
275.233603	10067.633033	28.060442
275.935690	10073.958404	28.065460
276.408711	10089.017868	28.070477
276.692820	10103.942574	28.075495
276.656974	10107.238144	28.080512
276.838713	10132.253846	28.085530
277.246034	10125.777945	28.090548
277.408118	10142.833935	28.095565
277.977547	10161.446236	28.100583
278.314024	10172.599298	28.105600
278.053459	10179.134566	28.110618
278.477560	10193.863896	28.115636
278.703203	10207.010731	28.120653
278.963016	10223.262243	28.125671
279.178633	10231.434676	28.130688
279.133569	10253.808421	28.135706
279.783561	10267.239699	28.140724
279.691696	10285.674074	28.145741
280.020956	10295.868498	28.150759
280.142077	10313.998209	28.155776
280.342201	10328.134200	28.160794
280.867830	10351.795824	28.165812
281.276443	10364.573288	28.170829
281.339123	10372.741178	28.175847
282.015420	10400.531354	28.180864
282.111049	10409.540307	28.185882
282.146392	10433.881426	28.190900
282.658565	10439.974427	28.195917
283.320522	10447.682794	28.200935
283.769128	10446.795244	28.205952
283.781856	10471.231496	28.210970
284.426072	10481.272793	28.215988
284.375733	10489.808800	28.221005
284.955728	10504.870892	28.226023
285.469849	10491.681403	28.231040
285.342566	10506.720999	28.236058
285.764416	10529.407584	28.241076
286.044814	10534.668416	28.246093
286.088962	10553.593379	28.251111
286.273030	10555.146636	28.256128
286.423505	10571.263919	28.261146
286.771389	10581.881849	28.266164
287.021430	10601.014769	28.271181
286.961369	10627.495932	28.276199
287.656561	10639.354365	28.281216
287.674566	10660.938896	28.286234
288.070422	10677.011753	28.291252
288.277628	10689.621880	28.296269
288.549168	10715.603187	28.301287
289.141717	10738.099265	28.306304
289.002099	10757.053044	28.311322
289.343219	10772.866123	28.316340
289.933992	10794.427943	28.321357
290.117010	10815.200758	28.326375
290.330441	10835.687849	28.331392
290.647978	10859.739308	28.336410
290.858293	10873.195273	28.341428
291.210046	10894.702854	28.346445
291.445842	10911.533363	28.351463
291.881677	10919.968617	28.356480
292.232023	10943.011001	28.361498
292.641288	10949.612758	28.366516
293.039976	10981.649614	28.371533
293.409417	10991.320338	28.376551
293.810057	11010.471278	28.381568
294.038900	11023.886578	28.386586
294.288343	11031.400498	28.391604
294.519004	11036.902870	28.396621
294.846522	11057.050378	28.401639
295.108217	11071.508883	28.406656
295.070619	11097.769347	28.411674
295.524677	11106.997537	28.416692
295.614475	11127.684173	28.421709
295.852249	11145.060833	28.426727
296.076973	11163.939356	28.431744
296.702061	11180.876849	28.436762
297.088586	11188.268450	28.441780
297.494965	11206.439871	28.446797
297.807876	11229.286356	28.451815
298.353327	11242.068380	28.456832
298.497491	11244.944593	28.461850
299.561914	11244.062175	28.466868
299.628955	11259.994118	28.471885
299.928542	11275.053126	28.476903
300.311256	11266.976642	28.481920
300.385159	11262.765683	28.486938
300.959433	11280.813154	28.491956
301.306348	11270.105708	28.496973
301.425880	11279.035579	28.501991
301.792909	11280.513050	28.507008
301.703153	11269.680978	28.512026
301.936855	11284.522909	28.517044
302.344941	11295.236073	28.522061
302.199438	11310.326514	28.527079
302.796547	11316.087671	28.532096
303.102754	11336.099867	28.537114
302.726241	11340.853795	28.542132
303.521950	11344.332718	28.547149
303.509371	11370.826486	28.552167
303.837688	11373.790878	28.557184
303.996605	11394.233390	28.562202
303.933324	11412.598117	28.567220
304.308338	11440.045213	28.572237
304.593297	11471.968000	28.577255
305.337084	11482.395348	28.582272
305.299576	11506.761836	28.587290
305.684441	11530.557386	28.592308
306.153787	11547.342636	28.597325
305.826611	11569.360863	28.602343
306.648108	11603.012789	28.607360
306.747599	11624.434181	28.612378
307.388954	11645.704928	28.617396
307.559850	11661.662093	28.622413
307.801416	11689.673436	28.627431
308.327971	11695.594103	28.632448
308.656937	11730.437570	28.637466
309.113248	11747.206082	28.642484
309.442602	11762.665023	28.647501
309.703464	11783.322593	28.652519
310.199290	11789.955379	28.657536
310.825671	11812.955861	28.662554
310.763200	11821.996425	28.667572
311.404732	11842.297979	28.672589
311.214866	11862.021684	28.677607
311.670311	11875.187598	28.682624
311.913980	11903.066312	28.687642
312.250404	11918.088527	28.692660
312.736212	11933.643241	28.697677
312.796997	11956.536181	28.702695
312.904518	11967.467037	28.707712
313.145113	11995.507406	28.712730
313.433375	12018.712349	28.717748
314.418177	12035.610404	28.722765
314.268259	12052.239905	28.727783
314.776291	12075.132828	28.732800
314.951280	12097.038758	28.737818
315.197973	12121.232332	28.742836
315.796229	12127.350380	28.747853
316.010367	12149.051342	28.752871
316.348964	12161.878832	28.757888
316.556820	12184.591269	28.762906
317.009663	12206.624584	28.767924
317.594225	12225.593409	28.772941
317.903068	12246.588207	28.777959
318.200945	12245.657733	28.782976
318.854508	12262.702294	28.787994
319.307855	12262.555985	28.793012
319.817396	12275.183266	28.798029
319.805320	12281.415330	28.803047
319.884352	12297.557853	28.808064
320.433266	12308.679120	28.813082
320.672109	12318.421387	28.818100
321.061629	12324.628836	28.823117
320.977471	12343.872406	28.828135
321.465811	12358.476610	28.833152
321.695537	12366.985658	28.838170
321.761499	12382.953457	28.843188
322.011190	12394.323453	28.848205
321.822520	12408.641539	28.853223
322.362266	12429.979520	28.858240
322.579302	12449.321562	28.863258
322.737650	12473.289356	28.868276
323.358819	12496.316751	28.873293
323.505187	12519.853861	28.878311
323.853269	12536.418888	28.883328
324.378937	12559.394916	28.888346
324.717272	12588.396696	28.893364
324.883128	12610.187808	28.898381
325.027618	12631.281251	28.903399
325.761674	12651.490335	28.908416
325.929291	12677.465279	28.913434
325.998964	12692.861208	28.918452
326.809454	12718.966641	28.923469
327.208324	12734.526081	28.928487
327.219276	12756.107804	28.933504
327.724017	12780.091532	28.938522
328.038511	12804.367004	28.943540
328.368204	12818.787852	28.948557
328.724135	12843.849528	28.953575
328.797150	12867.755322	28.958592
329.434184	12883.697794	28.963610
329.326949	12907.795906	28.968628
329.949467	12930.523632	28.973645
330.508248	12955.989654	28.978663
330.584991	12981.211816	28.983680
331.236335	13005.135113	28.988698
331.480168	13021.401016	28.993716
331.701050	13038.422067	28.998733
331.872495	13068.091604	29.003751
332.489477	13085.862593	29.008768
333.177635	13111.270789	29.013786
333.464006	13132.759538	29.018804
333.429430	13136.917531	29.023821
333.534302	13159.375603	29.028839
333.877103	13176.055698	29.033856
334.708465	13199.856481	29.038874
334.628570	13219.978161	29.043892
335.060198	13249.010643	29.048909
335.666259	13274.949729	29.053927
335.763395	13287.420846	29.058944
336.364973	13309.918608	29.063962
336.717863	13321.838357	29.068980
336.574368	13342.276382	29.073997
337.336670	13364.499716	29.079015
337.442047	13392.370585	29.084032
338.130220	13408.801328	29.089050
338.394827	13433.176955	29.094068
338.738753	13450.195011	29.099085
338.909116	13468.774839	29.104103
339.242116	13496.092529	29.109120
339.628319	13517.784069	29.114138
339.576860	13550.571178	29.119156
340.035276	13566.917828	29.124173
339.987733	13592.943317	29.129191
340.935644	13615.861213	29.134208
341.357851	13633.808307	29.139226
341.750179	13654.599043	29.144244
342.100710	13673.823661	29.149261
342.326841	13691.501332	29.154279
342.879230	13718.485185	29.159296
343.070075	13730.989375	29.164314
343.445278	13755.225039	29.169332
343.982028	13766.848020	29.174349
344.287787	13778.478548	29.179367
344.420344	13802.499413	29.184384
345.348816	13807.635010	29.189402
345.025416	13826.247849	29.194420
345.432532	13832.885698	29.199437
345.702140	13850.919914	29.204455
345.965428	13868.326698	29.209472
346.944714	13882.476698	29.214490
347.106235	13912.768065	29.219508
347.271740	13911.337057	29.224525
347.244425	13937.558822	29.229543
348.079984	13967.634812	29.234560
348.271309	13966.351363	29.239578
348.355067	13989.543199	29.244596
348.953323	14005.287390	29.249613
349.245052	14028.945857	29.254631
349.718279	14057.875207	29.259648
350.328657	14061.152970	29.264666
350.408779	14073.216715	29.269684
350.915778	14092.167917	29.274701
351.083353	14100.728478	29.279719
351.392359	14128.786631	29.284736
352.091899	14141.202422	29.289754
352.405594	14157.531060	29.294772
352.877686	14179.329992	29.299789
353.218451	14182.393952	29.304807
353.475737	14201.769418	29.309824
353.947026	14215.765063	29.314842
353.827079	14235.518252	29.319860
353.909977	14257.867358	29.324877
354.126069	14279.175711	29.329895
354.362424	14305.107450	29.334912
355.256767	14325.315483	29.339930
355.195087	14350.292585	29.344948
355.594767	14378.693849	29.349965
356.411789	14408.896590	29.354983
356.339611	14419.774732	29.360000
356.986074	14451.286263	29.365018
357.255217	14477.560519	29.370036
357.789082	14498.456469	29.375053
358.288747	14525.054922	29.380071
358.967725	14541.623881	29.385088
359.750501	14546.621305	29.390106
360.039864	14552.791398	29.395124
360.424223	14579.114177	29.400141
360.250458	14578.954957	29.405159
360.254276	14598.761890	29.410176
361.472518	14610.004541	29.415194
361.685473	14632.040138	29.420212
362.034746	14643.370722	29.425229
362.592045	14649.739147	29.430247
362.733076	14670.105882	29.435264
362.859421	14674.049673	29.440282
363.215257	14696.442072	29.445300
363.508862	14710.402583	29.450317
363.515737	14730.945015	29.455335
363.718392	14756.892092	29.460352
364.445046	14771.451590	29.465370
364.392152	14800.037635	29.470388
364.696530	14830.121895	29.475405
365.126603	14844.216007	29.480423
364.995512	14877.684166	29.485440
365.858245	14904.930890	29.490458
366.602043	14932.300388	29.495476
366.814241	14956.502959	29.500493
367.582598	14969.859183	29.505511
367.265427	14988.566930	29.510528
367.881464	15009.744358	29.515546
368.240883	15033.763043	29.520564
368.398259	15056.973142	29.525581
369.098214	15055.417790	29.530599
369.243565	15093.049954	29.535616
369.648300	15116.537433	29.540634
369.950872	15141.048302	29.545652
370.379807	15157.015619	29.550669
370.814787	15174.804275	29.555687
370.905254	15197.655456	29.560704
371.425689	15217.881596	29.565722
371.603103	15235.050347	29.570740
372.049670	15262.842419	29.575757
372.613861	15285.231497	29.580775
373.225800	15308.434299	29.585792
373.610021	15325.030882	29.590810
374.185980	15336.307639	29.595828
374.412890	15359.567288	29.600845
375.090411	15375.316069	29.605863
375.108631	15385.580629	29.610880
375.599818	15406.758987	29.615898
376.405426	15427.436794	29.620916
376.433537	15441.676041	29.625933
377.067458	15448.332840	29.630951
377.219385	15460.629468	29.635968
377.579644	15484.929673	29.640986
377.859391	15501.826916	29.646004
378.188915	15520.829283	29.651021
378.893321	15538.478429	29.656039
379.321117	15556.549644	29.661056
379.811917	15566.323841	29.666074
380.497800	15581.651446	29.671092
380.381294	15604.336366	29.676109
380.518006	15619.458939	29.681127
381.099895	15630.475971	29.686144
381.490612	15650.375359	29.691162
381.646827	15677.429991	29.696180
381.628185	15698.928073	29.701197
382.326414	15719.114434	29.706215
382.615461	15742.251178	29.711232
383.265150	15765.568674	29.716250
383.558812	15784.829549	29.721268
383.471420	15805.356230	29.726285
383.967982	15832.522325	29.731303
384.355903	15864.019597	29.736320
384.893677	15876.610152	29.741338
385.201234	15898.907256	29.746356
385.453308	15927.084304	29.751373
385.736682	15953.232047	29.756391
386.186079	15977.999064	29.761408
386.485438	16009.848302	29.766426
387.318560	16034.448270	29.771444
387.348546	16070.410619	29.776461
388.182136	16087.875930	29.781479
388.508836	16111.278874	29.786496
388.688421	16128.204898	29.791514
389.030977	16158.421117	29.796532
389.231116	16186.034971	29.801549
389.843050	16202.293666	29.806567
389.989192	16232.815357	29.811584
390.345208	16260.300825	29.816602
390.788358	16293.520984	29.821620
391.751208	16316.610374	29.826637
391.809826	16341.969304	29.831655
392.163226	16368.274105	29.836672
392.205812	16391.238391	29.841690
392.876116	16416.413757	29.846708
393.403509	16439.113122	29.851725
394.298288	16455.612254	29.856743
394.674267	16470.799318	29.861760
395.125833	16479.073540	29.866778
395.468117	16499.584604	29.871796
395.657681	16516.471516	29.876813
396.482081	16532.700575	29.881831
396.489806	16551.333997	29.886848
396.907307	16571.883963	29.891866
397.013900	16585.199062	29.896884
397.135338	16610.346428	29.901901
397.676804	16618.837279	29.906919
397.721375	16648.964850	29.911936
398.342370	16675.837988	29.916954
398.731974	16695.470170	29.921972
399.123023	16732.975712	29.926989
399.508149	16747.867837	29.932007
399.899163	16786.302069	29.937024
400.135603	16811.971889	29.942042
400.256744	16825.733389	29.947060
400.812199	16866.195172	29.952077
401.293610	16885.014166	29.957095
402.026591	16917.176418	29.962112
402.251025	16939.465564	29.967130
403.200202	16967.759865	29.972148
403.397722	17001.070024	29.977165
403.967442	17013.451055	29.982183
404.039616	17038.890914	29.987200
404.609509	17069.120552	29.992218
405.199047	17084.467522	29.997236
405.285192	17117.498324	30.002253
405.795169	17133.789477	30.007271
406.261765	17168.564639	30.012288
406.622538	17199.016547	30.017306
407.204743	17215.770302	30.022324
407.500305	17241.583099	30.027341
407.881150	17265.714956	30.032359
408.491838	17281.589423	30.037376
408.663851	17312.200396	30.042394
409.534440	17336.341377	30.047412
410.540923	17351.342542	30.052429
410.841492	17363.727799	30.057447
410.900001	17387.606771	30.062464
411.252797	17405.347126	30.067482
411.725472	17424.780766	30.072500
412.050429	17443.833129	30.077517
412.435387	17464.253299	30.082535
412.913561	17472.909153	30.087552
413.241735	17502.014754	30.092570
413.985411	17519.517483	30.097588
414.054218	17545.065925	30.102605
414.520463	17561.534812	30.107623
415.065400	17580.736261	30.112640
415.716096	17591.348893	30.117658
415.863053	17618.571945	30.122676
416.181059	17633.986897	30.127693
416.738011	17656.995800	30.132711
416.987036	17674.234550	30.137728
417.289779	17706.695681	30.142746
417.673691	17718.524913	30.147764
417.729571	17744.884233	30.152781
418.150928	17764.667335	30.157799
418.561461	17800.320981	30.162816
418.936610	17818.765766	30.167834
419.603243	17838.845572	30.172852
419.816207	17875.983079	30.177869
420.231905	17901.743313	30.182887
420.675815	17926.949588	30.187904
420.698794	17955.537991	30.192922
421.234561	17975.347718	30.197940
421.811475	18017.116253	30.202957
422.024489	18033.609173	30.207975
422.481229	18061.207880	30.212992
423.278589	18088.083963	30.218010
423.762344	18106.398403	30.223028
423.853105	18144.345113	30.228045
424.078359	18168.259105	30.233063
424.675467	18192.134187	30.238080
424.696430	18223.256554	30.243098
425.108944	18250.483375	30.248116
425.561479	18287.148475	30.253133
426.034554	18311.636848	30.258151
426.711690	18339.018436	30.263168
427.043019	18375.134007	30.268186
427.537029	18396.934333	30.273204
428.201834	18434.646944	30.278221
428.882904	18448.609874	30.283239
429.367196	18474.227526	30.288256
429.636539	18503.100572	30.293274
430.421789	18518.077076	30.298292
431.143808	18538.357465	30.303309
431.364258	18565.475645	30.308327
431.598722	18588.756975	30.313344
432.264525	18612.084897	30.318362
432.852828	18617.015761	30.323380
433.196231	18645.062534	30.328397
433.489247	18665.776258	30.333415
433.598650	18688.287490	30.338432
433.801862	18716.918449	30.343450
434.808946	18733.547363	30.348468
435.222331	18755.436455	30.353485
435.536980	18778.061141	30.358503
435.978032	18813.553965	30.363520
436.074929	18829.395980	30.368538
436.777586	18850.121939	30.373556
437.167797	18890.752676	30.378573
437.706848	18910.297513	30.383591
438.179550	18939.019515	30.388608
438.203945	18970.774304	30.393626
438.934815	18995.248679	30.398644
439.354320	19023.543173	30.403661
439.743327	19045.183682	30.408679
440.330908	19074.298645	30.413696
440.813686	19100.435406	30.418714
441.104197	19113.979480	30.423732
441.966895	19143.715069	30.428749
441.956272	19175.715716	30.433767
442.636438	19193.299347	30.438784
442.989738	19220.214547	30.443802
443.842104	19240.228989	30.448820
443.931492	19273.237691	30.453837
444.471168	19290.716928	30.458855
445.000554	19306.725758	30.463872
445.204316	19345.844952	30.468890
445.744996	19371.600319	30.473908
445.938106	19392.418820	30.478925
446.247422	19419.322189	30.483943
447.328530	19446.035949	30.488960
447.628485	19476.251356	30.493978
447.839630	19500.611429	30.498996
448.392932	19525.328920	30.504013
448.302057	19551.056489	30.509031
449.502100	19567.934066	30.514048
449.528374	19601.932407	30.519066
450.446596	19632.026534	30.524084
450.484877	19649.716825	30.529101
450.861503	19678.398017	30.534119
451.408246	19695.055200	30.539136
451.585762	19732.088054	30.544154
452.301099	19742.129522	30.549172
452.745576	19767.426551	30.554189
452.823933	19803.881099	30.559207
453.396787	19819.713002	30.564224
453.475130	19857.052154	30.569242
454.049819	19880.566369	30.574260
454.564229	19911.166045	30.579277
454.625134	19941.849007	30.584295
454.975126	19977.566621	30.589312
455.575649	20008.513165	30.594330
456.261605	20039.023156	30.599348
456.648816	20069.251170	30.604365
456.880028	20119.657827	30.609383
457.616115	20138.768875	30.614400
458.192471	20178.242401	30.619418
458.556680	20212.947354	30.624436
459.333746	20247.531233	30.629453
459.956699	20273.041217	30.634471
460.704690	20293.205674	30.639488
460.947546	20329.326009	30.644506
461.693598	20345.453596	30.649524
461.798738	20381.450152	30.654541
461.963344	20402.785930	30.659559
462.795954	20426.943002	30.664576
463.221617	20455.876742	30.669594
464.148863	20475.552261	30.674612
464.301608	20504.983463	30.679629
464.771581	20540.797153	30.684647
465.353956	20556.501812	30.689664
465.628103	20600.926092	30.694682
466.195334	20626.369396	30.699700
466.493067	20641.821483	30.704717
466.730293	20678.726788	30.709735
467.423448	20697.061618	30.714752
467.967058	20735.713689	30.719770
468.491123	20766.780746	30.724788
468.993475	20787.748455	30.729805
469.196088	20825.796698	30.734823
469.740000	20850.365694	30.739840
470.443784	20884.722017	30.744858
470.538865	20916.652191	30.749876
471.230985	20948.862247	30.754893
471.677784	20980.099627	30.759911
472.419671	21000.360539	30.764928
472.764821	21041.122813	30.769946
472.999829	21058.069786	30.774964
473.651449	21086.078404	30.779981
473.924861	21117.008126	30.784999
474.593986	21145.342655	30.790016
474.927720	21190.744649	30.795034
475.818710	21208.531058	30.800052
476.662347	21234.311221	30.805069
477.200102	21262.672689	30.810087
477.617361	21282.144091	30.815104
477.918012	21309.569515	30.820122
478.040252	21326.161492	30.825140
478.552269	21356.542659	30.830157
478.654150	21379.165573	30.835175
479.785473	21414.814718	30.840192
479.780286	21440.442968	30.845210
480.332015	21475.778076	30.850228
481.059065	21499.870769	30.855245
481.130870	21545.175353	30.860263
481.666120	21560.799696	30.865280
481.938692	21594.933746	30.870298
482.615834	21620.569738	30.875316
483.255106	21633.296732	30.880333
483.546524	21664.647849	30.885351
484.100027	21684.679739	30.890368
484.539999	21710.788746	30.895386
484.896401	21748.151392	30.900404
485.215654	21772.017253	30.905421
485.644909	21801.792779	30.910439
486.391647	21837.944860	30.915456
486.800684	21855.699473	30.920474
487.042127	21893.004468	30.925492
487.551045	21925.137230	30.930509
488.292676	21954.813809	30.935527
488.720379	21994.775387	30.940544
489.220185	22020.730163	30.945562
489.533306	22050.877985	30.950580
490.189517	22085.667162	30.955597
490.551382	22126.688144	30.960615
490.823933	22156.178989	30.965632
491.419163	22183.168014	30.970650
492.021443	22226.255881	30.975668
492.949553	22260.118426	30.980685
492.937024	22294.222246	30.985703
493.511256	22322.320498	30.990720
493.925530	22361.324470	30.995738
494.410115	22403.186263	31.000756
494.970670	22431.665921	31.005773
495.703812	22474.955113	31.010791
496.209997	22503.607626	31.015808
496.975083	22534.627317	31.020826
497.220399	22571.282159	31.025844
498.040637	22598.438924	31.030861
498.168165	22633.178676	31.035879
498.643425	22660.092249	31.040896
499.284166	22698.473983	31.045914
499.794474	22735.391177	31.050932
500.372501	22764.506795	31.055949
500.761209	22806.276948	31.060967
501.329901	22835.223515	31.065984
501.763270	22874.193931	31.071002
502.122182	22906.389556	31.076020
503.111610	22944.926007	31.081037
503.171620	22970.154319	31.086055
504.025473	23004.876433	31.091072
504.276888	23045.840688	31.096090
504.988312	23079.315005	31.101108
505.573958	23106.502671	31.106125
506.089384	23146.497152	31.111143
506.474340	23172.452363	31.116160
507.059583	23200.240520	31.121178
507.569077	23233.474818	31.126196
508.250048	23258.063395	31.131213
508.461171	23299.742172	31.136231
509.194625	23324.739715	31.141248
509.906042	23354.410463	31.146266
510.538324	23394.153448	31.151284
511.055379	23408.644667	31.156301
511.482533	23440.173357	31.161319
511.837789	23461.729206	31.166336
512.810408	23489.868201	31.171354
512.784583	23512.014230	31.176372
513.558988	23531.388020	31.181389
513.937372	23567.518462	31.186407
514.052556	23595.487774	31.191424
514.833595	23631.372395	31.196442
515.332832	23654.966063	31.201460
515.930348	23683.536555	31.206477
516.220661	23720.414002	31.211495
516.996745	23744.596590	31.216512
517.234203	23765.324344	31.221530
517.703352	23802.629080	31.226548
518.117263	23828.763897	31.231565
518.590338	23862.933835	31.236583
519.046332	23889.719374	31.241600
519.794800	23919.252496	31.246618
520.347454	23940.556963	31.251636
521.070639	23960.697450	31.256653
521.206648	23993.074879	31.261671
521.924581	24031.649390	31.266688
522.490307	24056.376963	31.271706
522.878968	24091.483041	31.276724
523.386461	24115.954346	31.281741
523.798803	24146.108865	31.286759
524.438938	24175.810896	31.291776
524.791453	24205.469277	31.296794
525.453232	24243.294628	31.301812
526.051574	24269.849982	31.306829
526.346400	24303.517604	31.311847
526.794500	24340.346356	31.316864
527.715436	24376.052559	31.321882
528.214913	24406.945908	31.326900
528.642363	24435.177433	31.331917
529.504339	24467.379422	31.336935
529.858779	24496.848356	31.341952
530.294095	24531.846836	31.346970
530.990395	24561.711322	31.351988
531.308975	24590.939522	31.357005
531.915717	24623.863992	31.362023
532.480618	24659.942100	31.367040
533.701136	24679.993254	31.372058
533.981463	24712.911811	31.377076
534.225012	24742.063440	31.382093
534.817124	24780.279821	31.387111
534.963168	24815.740915	31.392128
535.711862	24835.954151	31.397146
536.201355	24877.005178	31.402164
537.088167	24916.578868	31.407181
537.110912	24954.890539	31.412199
537.948433	24979.532708	31.417216
538.458722	25009.205638	31.422234
539.370722	25048.333301	31.427252
539.834990	25079.662900	31.432269
540.295731	25105.412926	31.437287
540.760380	25151.195413	31.442304
541.609565	25164.321737	31.447322
542.224428	25201.423135	31.452340
542.704983	25229.325216	31.457357
543.284796	25261.989507	31.462375
543.255172	25298.584734	31.467392
544.047085	25325.174554	31.472410
544.306146	25358.887437	31.477428
545.085172	25390.269635	31.482445
545.632497	25427.306130	31.487463
546.192737	25458.223242	31.492480
546.542465	25485.185456	31.497498
547.201534	25525.800634	31.502516
547.717708	25554.892045	31.507533
548.312504	25583.756388	31.512551
548.729369	25627.468216	31.517568
549.197045	25656.529406	31.522586
549.716748	25695.283343	31.527604
549.992016	25741.368406	31.532621
551.284411	25774.693611	31.537639
551.369843	25809.736152	31.542656
551.988208	25837.112043	31.547674
552.588950	25876.605768	31.552692
553.398764	25914.171080	31.557709
553.987569	25933.632980	31.562727
554.601130	25976.632406	31.567744
555.224063	25988.682206	31.572762
555.506941	26020.205827	31.577780
556.327361	26038.513160	31.582797
556.517900	26062.783395	31.587815
556.982612	26090.954574	31.592832
557.987968	26123.067390	31.597850
558.023271	26148.910266	31.602868
558.746382	26189.624254	31.607885
559.559157	26216.395286	31.612903
559.724623	26249.258405	31.617920
560.125266	26276.839426	31.622938
560.298222	26315.503179	31.627956
560.897375	26354.157538	31.632973
561.745615	26389.278255	31.637991
562.502496	26438.317199	31.643008
562.940157	26468.566071	31.648026
563.273438	26504.064194	31.653044
563.750007	26548.830487	31.658061
564.500570	26587.600762	31.663079
564.872088	26626.752442	31.668096
565.261308	26666.704088	31.673114
565.806534	26709.772597	31.678132
566.558179	26750.894081	31.683149
567.343909	26792.831953	31.688167
567.417770	26836.252195	31.693184
568.458332	26879.471478	31.698202
568.567122	26927.373760	31.703220
569.707255	26974.553107	31.708237
570.349975	27010.756045	31.713255
570.736515	27059.519182	31.718272
571.656143	27095.489559	31.723290
571.735144	27143.630836	31.728308
572.345199	27191.620033	31.733325
572.928334	27224.040501	31.738343
573.368211	27273.257226	31.743360
574.336223	27311.679028	31.748378
574.953966	27366.373227	31.753396
575.453405	27411.523404	31.758413
576.496524	27456.146625	31.763431
576.742737	27495.938881	31.768448
577.402975	27523.291581	31.773466
577.716115	27568.060289	31.778484
578.349934	27607.552251	31.783501
579.087817	27643.735185	31.788519
579.723186	27692.562234	31.793536
580.802381	27724.855718	31.798554
581.144175	27759.033756	31.803572
581.512472	27799.338514	31.808589
582.436176	27837.976785	31.813607
582.532482	27878.298760	31.818624
583.550844	27907.170014	31.823642
584.314975	27943.387320	31.828660
584.735207	27991.888314	31.833677
584.822667	28023.338028	31.838695
585.617985	28060.182735	31.843712
586.343386	28101.677634	31.848730
587.053354	28145.760109	31.853748
587.635532	28172.689723	31.858765
588.552570	28205.009216	31.863783
589.032692	28243.015734	31.868800
590.024712	28265.078060	31.873818
590.643653	28289.631902	31.878836
590.737440	28325.575011	31.883853
591.661778	28355.965836	31.888871
591.994057	28395.929751	31.893888
592.919100	28414.640116	31.898906
593.088965	28446.267272	31.903924
593.267082	28472.318415	31.908941
593.861677	28510.446666	31.913959
594.388257	28544.268584	31.918976
594.968392	28578.113825	31.923994
595.245401	28605.432833	31.929012
595.552911	28646.741073	31.934029
597.167992	28688.819226	31.939047
597.222781	28728.845953	31.944064
598.250219	28763.506765	31.949082
598.635934	28793.899925	31.954100
598.848884	28836.215620	31.959117
599.826352	28865.202056	31.964135
599.933003	28897.712013	31.969152
600.277838	28951.163526	31.974170
600.726183	28993.221674	31.979188
601.386819	29046.731727	31.984205
602.648605	29083.486707	31.989223
603.183351	29131.454278	31.994240
603.902041	29172.364567	31.999258
604.596176	29217.823444	32.004276
604.984076	29267.015152	32.009293
605.465685	29287.565192	32.014311
606.186441	29339.360019	32.019328
606.796270	29392.101417	32.024346
607.346045	29432.747761	32.029364
607.789168	29475.642073	32.034381
608.541829	29522.786523	32.039399
609.163979	29569.970360	32.044416
610.061945	29608.932046	32.049434
610.747665	29649.197362	32.054452
610.930455	29692.935419	32.059469
612.013861	29735.806452	32.064487
612.227609	29781.916575	32.069504
612.667009	29827.353249	32.074522
613.297351	29874.681896	32.079540
613.775855	29913.911734	32.084557
615.058105	29965.620733	32.089575
615.924353	30011.503373	32.094592
616.532642	30048.532490	32.099610
617.460105	30084.285693	32.104628
617.452410	30134.653578	32.109645
618.009707	30166.962648	32.114663
618.872841	30210.102846	32.119680
619.356676	30259.914113	32.124698
620.288359	30302.683527	32.129716
620.208995	30346.817770	32.134733
621.221432	30389.233449	32.139751
621.438750	30445.369927	32.144768
622.421388	30484.181027	32.149786
623.218028	30528.773484	32.154804
623.481824	30581.104030	32.159821
624.130917	30619.505857	32.164839
624.965384	30670.319184	32.169856
625.439088	30708.925477	32.174874
626.249143	30761.430615	32.179892
626.661529	30802.246446	32.184909
627.675859	30848.872781	32.189927
628.085660	30896.579462	32.194944
628.009627	30943.047040	32.199962
629.180573	30989.548170	32.204980
630.012468	31029.692291	32.209997
630.685136	31075.209189	32.215015
631.396599	31119.215649	32.220032
631.983254	31168.968855	32.225050
632.636035	31197.269528	32.230068
633.203907	31251.166403	32.235085
633.781263	31283.954532	32.240103
634.504017	31319.975644	32.245120
634.966665	31353.312745	32.250138
635.973482	31380.983301	32.255156
636.434443	31438.487921	32.260173
637.426809	31466.571739	32.265191
638.060559	31503.397217	32.270208
638.249810	31538.559852	32.275226
638.771193	31579.815401	32.280244
639.446470	31621.034432	32.285261
640.175411	31661.227415	32.290279
640.561647	31691.612132	32.295296
641.134920	31741.400404	32.300314
642.021183	31784.571902	32.305332
642.626402	31827.913674	32.310349
643.401246	31864.408069	32.315367
643.667941	31915.932366	32.320384
644.370984	31957.160386	32.325402
644.901693	31993.516006	32.330420
645.130090	32047.486763	32.335437
646.163365	32096.717507	32.340455
646.548745	32156.056536	32.345472
647.082995	32206.345093	32.350490
647.895050	32250.325653	32.355508
648.780105	32301.337407	32.360525
649.715890	32356.558028	32.365543
650.026981	32405.035840	32.370560
650.727154	32460.413529	32.375578
651.376698	32510.963035	32.380596
652.316121	32555.291080	32.385613
653.395128	32595.652642	32.390631
654.188665	32636.431714	32.395648
654.883397	32686.645874	32.400666
655.337023	32724.841801	32.405684
656.225173	32762.660381	32.410701
657.195804	32797.987992	32.415719
657.490212	32835.064637	32.420736
658.027426	32875.416255	32.425754
658.800354	32914.586981	32.430772
659.313057	32966.246272	32.435789
660.273219	33005.824239	32.440807
660.907968	33052.596809	32.445824
661.338477	33088.186011	32.450842
661.980264	33131.392042	32.455860
662.296999	33182.987546	32.460877
662.911698	33224.219184	32.465895
663.879724	33266.755148	32.470912
664.236260	33315.702156	32.475930
665.409521	33362.954255	32.480948
666.090289	33409.461254	32.485965
666.999932	33449.408288	32.490983
667.676168	33492.344173	32.496000
667.867812	33532.858333	32.501018
668.590512	33568.181590	32.506036
669.058285	33631.520239	32.511053
670.086273	33669.084774	32.516071
670.940338	33708.339191	32.521088
671.711011	33755.553694	32.526106
672.381365	33786.067936	32.531124
673.110367	33821.681463	32.536141
673.476685	33871.677739	32.541159
674.256242	33908.864109	32.546176
675.011808	33946.022668	32.551194
675.703254	33980.889961	32.556212
676.202541	34024.537291	32.561229
676.801487	34073.574779	32.566247
677.298859	34120.415376	32.571264
677.761009	34171.895841	32.576282
678.452672	34216.209080	32.581300
678.814014	34254.959567	32.586317
679.518008	34294.124641	32.591335
680.136649	34343.020599	32.596352
680.513917	34393.440012	32.601370
681.207648	34440.067404	32.606388
681.795597	34489.910523	32.611405
682.850691	34531.923385	32.616423
683.476521	34580.825099	32.621440
683.818911	34640.563533	32.626458
684.616736	34693.175323	32.631476
685.194281	34741.983768	32.636493
686.019909	34789.590360	32.641511
686.705083	34838.369628	32.646528
687.570819	34904.381500	32.651546
688.476453	34946.981166	32.656564
688.901087	34997.881490	32.661581
689.869800	35047.458008	32.666599
690.343315	35106.070891	32.671616
691.302050	35156.325739	32.676634
691.602768	35210.691706	32.681652
692.279095	35263.273251	32.686669
693.185255	35311.083455	32.691687
694.050782	35365.570545	32.696704
694.456480	35416.209270	32.701722
695.540733	35463.713896	32.706740
696.356114	35519.473736	32.711757
697.007169	35565.180815	32.716775
697.948742	35620.459714	32.721792
698.357952	35664.522797	32.726810
699.467707	35708.230327	32.731828
700.372685	35756.547547	32.736845
700.868717	35800.622688	32.741863
701.809633	35838.388017	32.746880
702.250052	35894.226182	32.751898
703.014011	35932.619898	32.756916
703.539180	35983.608108	32.761933
703.898062	36030.164680	32.766951
704.851663	36075.819441	32.771968
705.415817	36140.819869	32.776986
706.173936	36184.273298	32.782004
707.344435	36240.150473	32.787021
707.911809	36288.647920	32.792039
708.877955	36322.761826	32.797056
709.312627	36375.763130	32.802074
710.077421	36421.334212	32.807092
710.972456	36477.634275	32.812109
711.671520	36518.758059	32.817127
712.572857	36560.109680	32.822144
712.978494	36611.383573	32.827162
713.792693	36661.727725	32.832180
714.358146	36711.320330	32.837197
715.219302	36749.662454	32.842215
715.944203	36799.173535	32.847232
716.516432	36849.163763	32.852250
717.233935	36895.470385	32.857268
718.019060	36944.826996	32.862285
718.527020	36984.438575	32.867303
719.467357	37036.616671	32.872320
720.368732	37087.188540	32.877338
720.901640	37129.015952	32.882356
721.729590	37172.081135	32.887373
722.453874	37220.733330	32.892391
722.970027	37263.708124	32.897408
723.380190	37327.844565	32.902426
724.129491	37379.863540	32.907444
724.901827	37435.774221	32.912461
725.167106	37487.805573	32.917479
726.218014	37531.816891	32.922496
726.699395	37587.109308	32.927514
727.184994	37630.538554	32.932532
728.179165	37677.625842	32.937549
729.360759	37727.668705	32.942567
729.718255	37769.809231	32.947584
730.190754	37817.155090	32.952602
731.156868	37876.862434	32.957620
732.107154	37920.207283	32.962637
732.383947	37972.174784	32.967655
733.331397	38023.778747	32.972672
733.864575	38085.938025	32.977690
734.460174	38132.399097	32.982708
735.315284	38179.585019	32.987725
735.758313	38241.088484	32.992743
736.889859	38295.263424	32.997760
737.085889	38356.533756	33.002778
737.798224	38419.127730	33.007796
738.863593	38478.100405	33.012813
739.457907	38541.098848	33.017831
740.516496	38588.778856	33.022848
740.910641	38669.167282	33.027866
741.581380	38724.066376	33.032884
742.697991	38775.373893	33.037901
743.126615	38851.356327	33.042919
744.073518	38912.954015	33.047936
744.613954	38983.177540	33.052954
745.417991	39044.260322	33.057972
746.094846	39108.404828	33.062989
746.937855	39170.038394	33.068007
748.013090	39244.764295	33.073024
748.599118	39304.882583	33.078042
749.553506	39360.788904	33.083060
750.815017	39411.664328	33.088077
751.366970	39480.553335	33.093095
752.287482	39528.326481	33.098112
752.841707	39589.892369	33.103130
753.512256	39651.478268	33.108148
754.282122	39703.139197	33.113165
755.002850	39769.024252	33.118183
755.886417	39824.462173	33.123200
756.606099	39884.516998	33.128218
757.324387	39946.722384	33.133236
758.312842	40006.634523	33.138253
758.841956	40065.062606	33.143271
760.208255	40123.290958	33.148288
761.414555	40170.432893	33.153306
761.903654	40227.849460	33.158324
762.558171	40271.169192	33.163341
763.065973	40322.707965	33.168359
764.084313	40378.025135	33.173376
764.929254	40427.595449	33.178394
765.830200	40477.536610	33.183412
766.561733	40529.407849	33.188429
767.104546	40585.362428	33.193447
768.023442	40632.663943	33.198464
768.849791	40687.929575	33.203482
769.502597	40735.791326	33.208500
770.231132	40788.327700	33.213517
770.672360	40847.385024	33.218535
771.419734	40900.209653	33.223552
772.486500	40954.629021	33.228570
772.839961	41015.306847	33.233588
773.454116	41060.936504	33.238605
774.105105	41128.550444	33.243623
774.883029	41182.711774	33.248640
776.062376	41253.494601	33.253658
776.648592	41306.554008	33.258676
777.834503	41361.657860	33.263693
778.344203	41423.855668	33.268711
778.957959	41453.162723	33.273728
779.488316	41507.293827	33.278746
779.984984	41557.819007	33.283764
780.859137	41614.951605	33.288781
781.730823	41677.884353	33.293799
782.496309	41730.176908	33.298816
783.440901	41784.788129	33.303834
784.123282	41840.521812	33.308852
785.277331	41890.812612	33.313869
785.864248	41953.467926	33.318887
786.696873	42008.565158	33.323904
787.714641	42065.499485	33.328922
788.217319	42126.783306	33.333940
789.209997	42180.508897	33.338957
789.821145	42243.414255	33.343975
790.296131	42301.970596	33.348992
791.399633	42343.618067	33.354010
792.046782	42407.030594	33.359028
792.984166	42469.291287	33.364045
793.811426	42527.034417	33.369063
794.501951	42594.007919	33.374080
795.273308	42646.889954	33.379098
796.331084	42705.407247	33.384116
797.256916	42765.292432	33.389133
797.724081	42834.382318	33.394151
798.952830	42888.370162	33.399168
800.042694	42945.169049	33.404186
800.629016	43000.958578	33.409204
801.209097	43057.008543	33.414221
802.005492	43116.067287	33.419239
803.297329	43174.346992	33.424256
804.206982	43231.269545	33.429274
804.431498	43292.998386	33.434292
805.576524	43339.062470	33.439309
805.839841	43410.064424	33.444327
806.752538	43468.859331	33.449344
808.498912	43525.032535	33.454362
808.848088	43590.348101	33.459380
809.651461	43649.457786	33.464397
810.222342	43706.162317	33.469415
811.007168	43768.273323	33.474432
811.893670	43825.023904	33.479450
812.441812	43889.253075	33.484468
813.656235	43936.692819	33.489485
814.372420	44007.411135	33.494503
815.171000	44073.581650	33.499520
816.027941	44126.643664	33.504538
816.949592	44194.016155	33.509556
817.537417	44243.046862	33.514573
818.261362	44318.224290	33.519591
819.862704	44357.065535	33.524608
821.165037	44404.252235	33.529626
822.004904	44468.779240	33.534644
822.642832	44508.377956	33.539661
823.771195	44557.957751	33.544679
824.484138	44612.713244	33.549696
825.247493	44651.388159	33.554714
825.868377	44706.645270	33.559732
826.782054	44743.083047	33.564749
827.414740	44802.848594	33.569767
827.873163	44844.316557	33.574784
828.931628	44897.747547	33.579802
829.517418	44964.440901	33.584820
830.114675	45020.644968	33.589837
830.747131	45079.823021	33.594855
831.636683	45140.529945	33.599872
832.481452	45192.343939	33.604890
833.360205	45249.352388	33.609908
833.957413	45303.963131	33.614925
834.667645	45353.065786	33.619943
835.439687	45407.270029	33.624960
836.322847	45458.711781	33.629978
837.238379	45529.511435	33.634996
838.058662	45575.643368	33.640013
838.578967	45634.346945	33.645031
839.534158	45710.378667	33.650048
840.303749	45765.020633	33.655066
841.156660	45828.518448	33.660084
841.826466	45880.222107	33.665101
842.689424	45946.811988	33.670119
843.010809	46023.436844	33.675136
844.301452	46078.232518	33.680154
845.036246	46160.031258	33.685172
845.992678	46212.620964	33.690189
847.050544	46294.059935	33.695207
847.697795	46363.025201	33.700224
848.768794	46423.795924	33.705242
849.743466	46500.447230	33.710260
850.443421	46566.577226	33.715277
851.496532	46639.984238	33.720295
851.983645	46714.301975	33.725312
853.102257	46773.010283	33.730330
853.822312	46853.890244	33.735348
854.329767	46915.857075	33.740365
855.531279	46989.874731	33.745383
856.421847	47058.443666	33.750400
857.397148	47130.485302	33.755418
858.006877	47208.486351	33.760436
859.145954	47280.831932	33.765453
860.212266	47341.238944	33.770471
861.244287	47408.875955	33.775488
862.953654	47461.971342	33.780506
863.363060	47533.849307	33.785524
864.292228	47590.520561	33.790541
864.833976	47653.907481	33.795559
866.060084	47708.906961	33.800576
867.039308	47774.060735	33.805594
867.736049	47839.884974	33.810612
868.627444	47896.189621	33.815629
869.710336	47955.298798	33.820647
869.983474	48029.388459	33.825664
871.715070	48081.956756	33.830682
871.835353	48142.481539	33.835700
873.358807	48201.535431	33.840717
873.924791	48270.576107	33.845735
874.780882	48327.595881	33.850752
875.377019	48389.983140	33.855770
876.297336	48460.183915	33.860788
876.704034	48517.799218	33.865805
877.805546	48595.981547	33.870823
878.466747	48665.160435	33.875840
879.679027	48734.690282	33.880858
880.361621	48805.302393	33.885876
881.408124	48866.513702	33.890893
881.993727	48941.000550	33.895911
883.092055	49020.893018	33.900928
883.888407	49076.880074	33.905946
885.091295	49141.231101	33.910964
885.900142	49208.724742	33.915981
887.346900	49264.319986	33.920999
887.886662	49339.112625	33.926016
889.076534	49386.200757	33.931034
889.595870	49454.644914	33.936052
890.422434	49515.069721	33.941069
891.312616	49579.166975	33.946087
892.179256	49631.557162	33.951104
893.275651	49683.677612	33.956122
894.634025	49742.761202	33.961140
895.181716	49786.286889	33.966157
896.143488	49834.290884	33.971175
896.466006	49899.407447	33.976192
897.342845	49959.344759	33.981210
898.306571	50026.639551	33.986228
899.369026	50085.763763	33.991245
900.068873	50140.041193	33.996263
900.666168	50198.991355	34.001280
901.334399	50262.859338	34.006298
902.470449	50342.219082	34.011316
902.984887	50404.656189	34.016333
904.101464	50476.199240	34.021351
904.814928	50551.778652	34.026368
905.967842	50622.778702	34.031386
906.682037	50699.914947	34.036404
907.561988	50773.900052	34.041421
908.344504	50846.609827	34.046439
909.135799	50930.523857	34.051456
910.204298	51003.866616	34.056474
911.240941	51081.700551	34.061492
911.910155	51159.990558	34.066509
913.320710	51233.021384	34.071527
913.888767	51321.773961	34.076544
914.999677	51392.333683	34.081562
916.204027	51481.202952	34.086580
916.890431	51553.050415	34.091597
918.056266	51614.237821	34.096615
918.385858	51697.910139	34.101632
919.648051	51769.864793	34.106650
920.828371	51853.626704	34.111668
921.754455	51936.783095	34.116685
922.470032	52017.719977	34.121703
923.680567	52084.444518	34.126720
924.658893	52154.577950	34.131738
925.132009	52241.836555	34.136756
926.384576	52315.104195	34.141773
927.528155	52393.020802	34.146791
927.853570	52470.058943	34.151808
929.333833	52548.575402	34.156826
930.382880	52620.705080	34.161844
931.044810	52699.539261	34.166861
932.507390	52764.106761	34.171879
933.405140	52843.948785	34.176896
934.300866	52910.250123	34.181914
935.130916	52985.135928	34.186932
936.091355	53058.109683	34.191949
937.700637	53128.565463	34.196967
938.696476	53198.591741	34.201984
939.491545	53255.475019	34.207002
940.297428	53327.657390	34.212020
940.915364	53396.243394	34.217037
942.301366	53465.152989	34.222055
942.940623	53539.620992	34.227072
943.710450	53597.654375	34.232090
944.672923	53674.806140	34.237108
945.576897	53754.340237	34.242125
946.706136	53813.520513	34.247143
947.494709	53895.914298	34.252160
948.959114	53959.662185	34.257178
949.869035	54019.617495	34.262196
950.905612	54088.153012	34.267213
951.963883	54150.661066	34.272231
953.004661	54218.544523	34.277248
953.816841	54273.098886	34.282266
954.772621	54325.530100	34.287284
955.840655	54392.599823	34.292301
956.667008	54431.281488	34.297319
957.375031	54492.395835	34.302336
958.300179	54540.010267	34.307354
959.513232	54602.160038	34.312372
960.094383	54663.300906	34.317389
960.983963	54721.539910	34.322407
961.882512	54779.454925	34.327424
962.960711	54837.437040	34.332442
963.822602	54894.839131	34.337460
964.859093	54966.705869	34.342477
966.055214	55020.297258	34.347495
966.920210	55085.685600	34.352512
967.851730	55151.133379	34.357530
968.658599	55209.139658	34.362548
969.072020	55283.350899	34.367565
970.554598	55348.010999	34.372583
971.507249	55430.485861	34.377600
972.287905	55496.723812	34.382618
973.268646	55576.707753	34.387636
974.200917	55638.998886	34.392653
975.017180	55719.920206	34.397671
976.202233	55797.493591	34.402688
977.386151	55866.618871	34.407706
978.242740	55940.339174	34.412724
978.845013	56017.320514	34.417741
980.168876	56084.829856	34.422759
980.665587	56165.555622	34.427776
981.947344	56235.717289	34.432794
983.470113	56320.675904	34.437812
983.668387	56398.436496	34.442829
984.758394	56472.128441	34.447847
985.806925	56555.358048	34.452864
986.799662	56635.109521	34.457882
988.018507	56706.225343	34.462900
988.866793	56793.644916	34.467917
990.122216	56867.635100	34.472935
990.677125	56943.664832	34.477952
991.808430	57028.883098	34.482970
993.262625	57112.450216	34.487988
994.023103	57190.885330	34.493005
995.463169	57271.398373	34.498023
996.022856	57347.783061	34.503040
997.121926	57427.969977	34.508058
997.871312	57502.857324	34.513076
998.822507	57591.959944	34.518093
999.589450	57672.971510	34.523111
1000.819258	57767.417364	34.528128
1001.636088	57847.440758	34.533146
1002.914602	57931.246935	34.538164
1003.871881	58019.831214	34.543181
1004.738998	58090.347674	34.548199
1005.792186	58185.531519	34.553216
1006.759462	58267.463267	34.558234
1007.976014	58348.578007	34.563252
1008.687369	58436.917289	34.568269
1009.854393	58519.628935	34.573287
1010.859729	58617.385255	34.578304
1012.095143	58693.896881	34.583322
1013.403775	58766.568154	34.588340
1014.539749	58855.608710	34.593357
1015.278207	58940.040448	34.598375
1016.662768	59024.093418	34.603392
1017.677898	59090.741534	34.608410
1018.696371	59174.763401	34.613428
1019.860912	59250.540957	34.618445
1021.299771	59306.806823	34.623463
1021.978438	59389.331627	34.628480
1022.733674	59446.710608	34.633498
1023.725162	59507.451863	34.638516
1024.884928	59582.104557	34.643533
1025.839934	59630.363763	34.648551
1026.858885	59698.487725	34.653568
1028.060097	59763.728896	34.658586
1029.128678	59827.535095	34.663604
1030.085755	59893.599479	34.668621
1030.764980	59963.479713	34.673639
1032.031628	60017.299174	34.678656
1032.861147	60079.522875	34.683674
1034.387766	60150.733879	34.688692
1034.873217	60228.082332	34.693709
1035.581149	60291.692701	34.698727
1036.820480	60376.159068	34.703744
1037.797158	60461.514790	34.708762
1038.866548	60539.273380	34.713780
1039.824291	60629.449549	34.718797
1040.811389	60693.137775	34.723815
1042.115864	60771.942900	34.728832
1042.694729	60851.494206	34.733850
1043.706862	60929.573109	34.738868
1044.698141	61022.309081	34.743885
1045.977396	61098.777144	34.748903
1046.700150	61185.232002	34.753920
1047.342042	61277.497944	34.758938
1048.625985	61362.239286	34.763956
1049.876003	61465.020232	34.768973
1050.870926	61547.528419	34.773991
1051.806284	61643.079619	34.779008
1052.738205	61737.783501	34.784026
1053.894161	61818.697685	34.789044
1055.142298	61923.164630	34.794061
1056.266831	62014.978404	34.799079
1057.342311	62104.825160	34.804096
1058.317301	62189.908628	34.809114
1059.774783	62297.142492	34.814132
1060.582247	62390.836438	34.819149
1061.993518	62475.833990	34.824167
1063.518545	62561.871277	34.829184
1064.652399	62634.283742	34.834202
1065.713555	62714.215439	34.839220
1066.904624	62795.513506	34.844237
1067.790170	62875.295809	34.849255
1069.390738	62946.091942	34.854272
1070.303742	63030.694186	34.859290
1071.469864	63106.958196	34.864308
1072.388075	63194.054353	34.869325
1073.604842	63266.569707	34.874343
1074.686781	63342.410747	34.879360
1075.267171	63431.149257	34.884378
1076.526569	63513.812751	34.889396
1077.583361	63591.437328	34.894413
1078.949630	63673.040183	34.899431
1080.017792	63747.282981	34.904448
1080.921180	63829.312909	34.909466
1082.330841	63902.369842	34.914484
1083.376065	63979.136470	34.919501
1084.221182	64061.745987	34.924519
1085.460774	64127.429563	34.929536
1086.091250	64211.440401	34.934554
1087.401967	64297.295485	34.939572
1088.178623	64385.829581	34.944589
1089.227044	64456.696968	34.949607
1090.396870	64543.404151	34.954624
1091.163714	64633.111834	34.959642
1092.035107	64717.802246	34.964660
1093.096831	64811.946862	34.969677
1094.357231	64897.140769	34.974695
1095.396040	64965.390129	34.979712
1096.680954	65039.824604	34.984730
1097.539828	65120.390600	34.989748
1098.453169	65202.448801	34.994765
1099.234650	65290.877712	34.999783
1100.210937	65370.368968	35.004800
1101.150036	65469.682193	35.009818
1102.610944	65561.709914	35.014836
1103.628441	65657.637257	35.019853
1104.680865	65748.171812	35.024871
1106.073905	65823.889639	35.029888
1106.766405	65930.080605	35.034906
1108.186258	66020.520957	35.039924
1109.352380	66106.708621	35.044941
1110.458947	66203.314265	35.049959
1111.684087	66281.921281	35.054976
1112.553054	66378.532920	35.059994
1114.118131	66474.232509	35.065012
1114.906259	66574.852480	35.070029
1116.141954	66670.217873	35.075047
1117.758437	66752.969398	35.080064
1118.873504	66840.838967	35.085082
1120.066863	66926.828910	35.090100
1121.703899	67005.494350	35.095117
1122.952266	67092.793213	35.100135
1124.332993	67165.047373	35.105152
1124.838872	67257.888380	35.110170
1126.226100	67339.081983	35.115188
1127.278841	67426.659367	35.120205
1128.712613	67505.041418	35.125223
1130.019934	67591.838960	35.130240
1130.601585	67673.684536	35.135258
1131.512506	67755.320832	35.140276
1132.863281	67834.318310	35.145293
1133.859679	67934.961885	35.150311
1135.454116	68016.125388	35.155328
1136.042670	68100.959772	35.160346
1137.395906	68184.124157	35.165364
1138.403229	68271.990098	35.170381
1139.399778	68380.125760	35.175399
1140.831905	68455.104529	35.180416
1142.048730	68552.885942	35.185434
1142.989586	68643.093578	35.190452
1144.610694	68732.524477	35.195469
1145.319407	68824.206196	35.200487
1146.726793	68905.350975	35.205504
1147.826397	69015.467791	35.210522
1148.797781	69092.381700	35.215540
1150.065624	69187.504530	35.220557
1151.041378	69277.189739	35.225575
1152.417013	69366.914326	35.230592
1153.075198	69457.428420	35.235610
1154.445392	69554.195642	35.240628
1155.515956	69647.273983	35.245645
1156.824487	69744.488424	35.250663
1158.040511	69837.202877	35.255680
1159.303186	69931.613728	35.260698
1160.367613	70026.277405	35.265716
1161.621875	70116.055142	35.270733
1162.721409	70211.017970	35.275751
1164.073346	70288.566402	35.280768
1165.217076	70388.430424	35.285786
1166.415144	70478.484113	35.290804
1167.371347	70570.481762	35.295821
1168.758304	70648.545060	35.300839
1170.064057	70740.754856	35.305856
1171.060987	70832.139192	35.310874
1172.111619	70911.547417	35.315892
1173.400734	71000.974506	35.320909
1173.977490	71076.556277	35.325927
1175.405970	71146.458536	35.330944
1176.132735	71238.380271	35.335962
1176.938642	71319.879524	35.340980
1178.066451	71401.024970	35.345997
1179.390050	71499.364459	35.351015
1180.343718	71586.249458	35.356032
1181.436187	71692.123298	35.361050
1182.494521	71797.508942	35.366068
1183.932167	71895.198912	35.371085
1185.002793	71998.379721	35.376103
1186.286491	72093.232067	35.381120
1187.507967	72201.646249	35.386138
1188.198117	72302.417750	35.391156
1189.752281	72411.743575	35.396173
1190.892604	72509.279459	35.401191
1192.244850	72611.975548	35.406208
1193.611716	72722.421043	35.411226
1194.862065	72818.750389	35.416244
1196.316855	72923.179572	35.421261
1197.641978	73028.617271	35.426279
1198.923279	73113.391810	35.431296
1200.143818	73214.818843	35.436314
1201.514520	73317.704786	35.441332
1203.466998	73396.232858	35.446349
1204.421825	73488.354926	35.451367
1206.228292	73567.932169	35.456384
1207.098522	73665.919666	35.461402
1208.464063	73749.568525	35.466420
1209.999585	73847.934446	35.471437
1210.839016	73932.324404	35.476455
1211.891367	74016.478830	35.481472
1213.198156	74113.234741	35.486490
1213.996071	74201.153204	35.491508
1215.263601	74302.083090	35.496525
1216.338506	74406.095919	35.501543
1217.777952	74499.843337	35.506560
1218.706324	74594.721944	35.511578
1219.524975	74698.395805	35.516596
1220.705350	74793.577886	35.521613
1222.154650	74900.358985	35.526631
1223.249282	75018.734972	35.531648
1224.671208	75121.404573	35.536666
1225.740053	75223.027523	35.541684
1226.831504	75330.182700	35.546701
1228.271499	75443.630112	35.551719
1229.346950	75541.972542	35.556736
1230.679766	75644.100669	35.561754
1231.811758	75757.508677	35.566772
1232.918548	75869.312377	35.571789
1234.292619	75975.830784	35.576807
1235.787318	76071.994496	35.581824
1237.078291	76183.517487	35.586842
1238.309534	76290.692724	35.591860
1239.565151	76395.141137	35.596877
1240.659852	76492.090637	35.601895
1242.229390	76593.463474	35.606912
1244.038997	76692.417857	35.611930
1245.439076	76788.788855	35.616948
1246.963213	76880.428592	35.621965
1247.936427	76978.361467	35.626983
1248.935382	77070.400278	35.632000
1250.461305	77162.826078	35.637018
1251.542187	77259.159756	35.642036
1252.684961	77347.389496	35.647053
1253.892667	77437.344892	35.652071
1255.258292	77530.531619	35.657088
1256.344481	77605.558532	35.662106
1257.143907	77691.689304	35.667124
1258.472617	77776.192482	35.672141
1259.015926	77873.625435	35.677159
1260.112355	77965.196049	35.682176
1261.558579	78068.848473	35.687194
1262.573819	78169.743396	35.692212
1264.308685	78256.021707	35.697229
1265.604371	78353.782641	35.702247
1266.732825	78454.052918	35.707264
1268.785510	78545.501966	35.712282
1269.582859	78651.803907	35.717300
1270.982828	78738.883293	35.722317
1272.079195	78835.448140	35.727335
1273.361279	78932.136439	35.732352
1274.694550	79038.280445	35.737370
1275.768718	79144.021792	35.742388
1277.240548	79247.446645	35.747405
1278.303173	79349.212650	35.752423
1279.977705	79449.363548	35.757440
1281.305017	79550.747043	35.762458
1282.915068	79651.326776	35.767476
1284.518314	79738.022954	35.772493
1285.958394	79835.411945	35.777511
1287.353210	79926.587912	35.782528
1288.876496	80018.453641	35.787546
1289.736035	80116.668778	35.792564
1291.459468	80203.943148	35.797581
1292.423049	80300.533780	35.802599
1293.688407	80388.374121	35.807616
1295.174728	80497.071720	35.812634
1296.276228	80595.694307	35.817652
1297.499068	80691.637822	35.822669
1298.454039	80788.307501	35.827687
1299.326506	80893.871535	35.832704
1301.000762	80991.076093	35.837722
1301.842764	81098.241978	35.842740
1303.055302	81203.678233	35.847757
1304.480680	81320.002858	35.852775
1305.788084	81437.461250	35.857792
1306.593856	81552.185561	35.862810
1307.944645	81665.913295	35.867828
1309.447939	81784.330880	35.872845
1310.635826	81896.159107	35.877863
1312.093907	82013.000974	35.882880
1313.779777	82130.644082	35.887898
1314.676510	82254.061292	35.892916
1316.403582	82358.167472	35.897933
1318.119700	82470.878678	35.902951
1319.425793	82579.536385	35.907968
1320.669345	82694.577310	35.912986
1321.858383	82806.396296	35.918004
1323.651720	82913.167613	35.923021
1324.606033	83023.896345	35.928039
1325.765796	83139.256204	35.933056
1327.732685	83237.525294	35.938074
1328.678626	83344.822916	35.943092
1330.472661	83448.605927	35.948109
1331.756548	83552.380028	35.953127
1332.922479	83657.642651	35.958144
1334.133297	83764.343123	35.963162
1335.643218	83872.505245	35.968180
1336.623150	83974.275551	35.973197
1338.037104	84082.985577	35.978215
1339.603117	84199.046742	35.983232
1340.855730	84300.535023	35.988250
1341.893580	84400.523917	35.993268
1343.210910	84495.642041	35.998285
1344.942927	84597.690303	36.003303
1345.642960	84686.772401	36.008320
1347.373633	84787.681159	36.013338
1348.486801	84889.395968	36.018356
1349.496683	84989.049147	36.023373
1350.814236	85091.999973	36.028391
1352.143239	85193.150073	36.033408
1353.486762	85308.730840	36.038426
1354.359785	85423.168858	36.043444
1355.902075	85524.565692	36.048461
1356.992825	85634.649724	36.053479
1358.233141	85757.521745	36.058496
1360.169353	85870.921721	36.063514
1361.103343	85997.289093	36.068532
1362.624207	86114.543473	36.073549
1363.743712	86229.149060	36.078567
1365.173513	86356.479901	36.083584
1366.667338	86477.541476	36.088602
1367.707495	86599.877992	36.093620
1369.505649	86734.021289	36.098637
1371.105035	86852.698351	36.103655
1372.099111	86978.186270	36.108672
1374.041232	87083.061810	36.113690
1375.157896	87212.092499	36.118708
1377.111949	87328.017135	36.123725
1378.544726	87440.994712	36.128743
1379.883562	87563.744978	36.133760
1381.480169	87671.806457	36.138778
1383.101817	87786.606126	36.143796
1384.403402	87897.008050	36.148813
1386.403417	88019.302486	36.153831
1387.522874	88129.987083	36.158848
1389.218216	88225.730244	36.163866
1390.816459	88339.281136	36.168884
1392.436443	88448.102189	36.173901
1393.719142	88551.653617	36.178919
1394.784694	88659.218442	36.183936
1396.366337	88766.906095	36.188954
1397.166191	88872.320662	36.193972
1398.643898	88984.815611	36.198989
1400.131967	89101.567472	36.204007
1401.586553	89222.481737	36.209024
1403.154198	89326.865964	36.214042
1404.297236	89441.797264	36.219060
1405.837517	89548.024121	36.224077
1407.841076	89649.908400	36.229095
1409.619846	89755.161065	36.234112
1410.988429	89848.121546	36.239130
1412.363705	89961.713366	36.244148
1413.848024	90051.754288	36.249165
1415.338107	90160.842644	36.254183
1416.482749	90264.535600	36.259200
1417.822687	90364.966789	36.264218
1419.350045	90468.854354	36.269236
1420.108493	90586.701465	36.274253
1421.698735	90694.825664	36.279271
1423.045396	90809.857277	36.284288
1424.484339	90909.476443	36.289306
1425.762410	91022.719886	36.294324
1427.162808	91132.763598	36.299341
1428.365965	91250.404684	36.304359
1429.196932	91371.766909	36.309376
1431.263171	91488.653570	36.314394
1432.214891	91605.676134	36.319412
1433.365160	91720.703775	36.324429
1434.982991	91854.784254	36.329447
1435.996186	91981.025432	36.334464
1437.704776	92087.285789	36.339482
1438.908188	92207.135868	36.344500
1440.119556	92319.697476	36.349517
1441.644180	92431.133427	36.354535
1442.533656	92553.530577	36.359552
1443.797968	92672.156273	36.364570
1445.686080	92805.590515	36.369588
1447.239764	92930.446042	36.374605
1448.532183	93035.101454	36.379623
1449.802883	93165.997063	36.384640
1451.294039	93289.862498	36.389658
1453.180315	93418.939622	36.394676
1454.870252	93541.292194	36.399693
1456.026128	93672.499361	36.404711
1457.204765	93790.052698	36.409728
1459.004302	93906.774699	36.414746
1460.563477	94048.846493	36.419764
1462.091526	94177.006592	36.424781
1463.743464	94296.744357	36.429799
1465.254988	94428.735952	36.434816
1466.741942	94549.197510	36.439834
1468.143282	94683.362128	36.444852
1469.460156	94813.433677	36.449869
1471.079250	94941.303924	36.454887
1472.431024	95077.810231	36.459904
1474.055608	95204.223037	36.464922
1476.039416	95328.527014	36.469940
1477.688931	95454.214454	36.474957
1479.809107	95564.580388	36.479975
1481.044077	95685.567259	36.484992
1482.530005	95807.897190	36.490010
1484.328610	95929.114172	36.495028
1486.035253	96043.577060	36.500045
1487.680754	96151.635907	36.505063
1488.478670	96275.063472	36.510080
1489.942891	96391.416048	36.515098
1491.906175	96517.920904	36.520116
1493.015179	96642.163463	36.525133
1494.992816	96757.245939	36.530151
1495.846558	96880.160153	36.535168
1497.644436	97004.372983	36.540186
1499.433202	97126.179236	36.545204
1500.499763	97249.289939	36.550221
1502.012185	97365.004805	36.555239
1503.436936	97502.816004	36.560256
1504.846441	97620.335195	36.565274
1506.650484	97740.138566	36.570292
1508.474632	97865.833849	36.575309
1510.189850	97974.775469	36.580327
1511.208788	98101.116752	36.585344
1512.819020	98214.271500	36.590362
1514.529274	98333.217021	36.595380
1515.973021	98467.670128	36.600397
1517.475563	98587.029231	36.605415
1519.018083	98715.154954	36.610432
1520.552784	98827.081305	36.615450
1522.084476	98950.645969	36.620468
1523.811508	99063.760203	36.625485
1525.264618	99177.906283	36.630503
1526.538801	99309.334158	36.635520
1527.997072	99427.410227	36.640538
1529.747222	99549.510684	36.645556
1530.911290	99679.042955	36.650573
1532.499884	99799.204533	36.655591
1533.708025	99931.481935	36.660608
1535.251014	100052.044553	36.665626
1536.787993	100183.359035	36.670644
1538.261570	100293.373044	36.675661
1539.725833	100409.119125	36.680679
1540.904391	100532.187023	36.685696
1541.909686	100659.884340	36.690714
1543.686532	100775.354882	36.695732
1545.484788	100906.175236	36.700749
1547.003422	101017.503178	36.705767
1548.215317	101144.612424	36.710784
1549.603025	101278.401400	36.715802
1551.265715	101400.978870	36.720820
1552.937093	101530.325489	36.725837
1554.476659	101658.907099	36.730855
1555.666787	101789.597452	36.735872
1557.369727	101915.758489	36.740890
1559.016825	102054.581525	36.745908
1560.369356	102205.482643	36.750925
1562.312055	102338.859946	36.755943
1563.780969	102475.392369	36.760960
1565.254520	102618.606153	36.765978
1566.767611	102752.533780	36.770996
1568.257800	102894.820649	36.776013
1569.674672	103036.904007	36.781031
1571.206559	103184.130270	36.786048
1572.909405	103329.707711	36.791066
1574.868997	103477.363178	36.796084
1576.258143	103631.498197	36.801101
1578.116979	103760.215827	36.806119
1579.463624	103916.273287	36.811136
1580.798488	104064.041277	36.816154
1582.704442	104214.472380	36.821172
1584.389112	104365.597916	36.826189
1586.395372	104501.129482	36.831207
1587.854990	104656.627620	36.836224
1589.163426	104793.625655	36.841242
1591.030390	104942.950334	36.846260
1592.483072	105106.794608	36.851277
1593.964478	105246.810615	36.856295
1595.645840	105395.709736	36.861312
1597.433369	105546.811906	36.866330
1599.501703	105677.355516	36.871348
1601.291926	105834.341871	36.876365
1603.465341	105968.458584	36.881383
1605.039067	106120.002345	36.886400
1606.081157	106248.463577	36.891418
1607.911207	106391.397131	36.896436
1609.471419	106539.457918	36.901453
1611.146298	106680.489498	36.906471
1612.724038	106821.118342	36.911488
1614.131769	106969.230090	36.916506
1616.316892	107115.547712	36.921524
1617.455808	107257.692186	36.926541
1618.830850	107390.696115	36.931559
1620.500592	107540.443343	36.936576
1621.916744	107701.123080	36.941594
1623.771244	107837.249556	36.946612
1625.383207	107989.340921	36.951629
1626.943244	108135.886993	36.956647
1628.559406	108281.359788	36.961664
1629.900791	108439.188807	36.966682
1631.725145	108574.156273	36.971700
1633.360152	108735.871942	36.976717
1634.767946	108881.582584	36.981735
1636.821605	109041.421172	36.986752
1638.202888	109187.644456	36.991770
1640.195949	109337.349154	36.996788
1641.834325	109491.611442	37.001805
1643.311362	109621.323711	37.006823
1644.917848	109776.086779	37.011840
1646.353194	109924.600013	37.016858
1648.335983	110061.843875	37.021876
1649.130454	110187.961578	37.026893
1650.979463	110332.582429	37.031911
1652.195551	110472.470801	37.036928
1654.102136	110612.734152	37.041946
1656.173272	110740.189580	37.046964
1657.951343	110887.220540	37.051981
1659.329518	111023.167297	37.056999
1661.016969	111166.650019	37.062016
1662.562022	111312.729855	37.067034
1664.542702	111445.908639	37.072052
1666.330383	111586.803084	37.077069
1667.662086	111733.513900	37.082087
1669.522800	111877.492483	37.087104
1671.014238	112021.922261	37.092122
1672.870112	112163.150786	37.097140
1674.734068	112310.656190	37.102157
1676.367948	112458.134602	37.107175
1677.856793	112614.754613	37.112192
1679.203868	112762.342326	37.117210
1681.260976	112901.158202	37.122228
1682.666665	113052.656781	37.127245
1683.831363	113219.462988	37.132263
1686.234055	113380.839472	37.137280
1687.485212	113537.665365	37.142298
1689.135213	113695.355682	37.147316
1690.698849	113869.369851	37.152333
1692.561572	114030.896690	37.157351
1694.097009	114200.604759	37.162368
1695.658198	114363.651194	37.167386
1697.878018	114537.680579	37.172404
1699.392446	114711.135709	37.177421
1701.299525	114874.625225	37.182439
1703.371915	115033.346326	37.187456
1704.872726	115212.145464	37.192474
1707.044198	115373.186287	37.197492
1708.612870	115537.428995	37.202509
1710.501005	115698.477291	37.207527
1712.346563	115861.968096	37.212544
1713.498391	116026.873973	37.217562
1715.218023	116181.520184	37.222580
1717.031687	116362.774825	37.227597
1718.484591	116532.011860	37.232615
1720.596014	116693.638541	37.237632
1721.767927	116867.613731	37.242650
1723.677564	117036.350732	37.247668
1725.509013	117213.662146	37.252685
1727.277835	117395.144413	37.257703
1729.443594	117549.156103	37.262720
1730.869297	117733.331639	37.267738
1732.945844	117895.590457	37.272756
1734.587672	118063.092690	37.277773
1736.075256	118242.555338	37.282791
1738.234613	118403.535053	37.287808
1739.284142	118580.682878	37.292826
1741.365986	118756.668812	37.297844
1742.879989	118934.266051	37.302861
1744.629841	119102.720077	37.307879
1746.589565	119273.476108	37.312896
1748.210110	119454.040016	37.317914
1749.946894	119613.809504	37.322932
1751.779995	119784.016726	37.327949
1753.445796	119956.927191	37.332967
1755.488541	120132.532338	37.337984
1757.203159	120310.041324	37.343002
1758.992006	120474.055670	37.348020
1761.136816	120655.596474	37.353037
1762.614149	120810.717936	37.358055
1764.134134	120955.139992	37.363072
1765.706731	121122.400033	37.368090
1767.657257	121272.756258	37.373108
1769.143900	121444.280547	37.378125
1770.676369	121591.430321	37.383143
1772.485202	121745.045133	37.388160
1773.636979	121911.663692	37.393178
1775.472605	122087.195768	37.398196
1777.228490	122256.258830	37.403213
1778.776114	122436.606984	37.408231
1780.776080	122609.933933	37.413248
1782.140627	122795.627434	37.418266
1784.091775	122976.118225	37.423284
1785.982153	123152.724810	37.428301
1787.408885	123340.022267	37.433319
1789.563894	123524.657424	37.438336
1791.242237	123714.112122	37.443354
1792.954534	123896.483720	37.448372
1795.229095	124077.563481	37.453389
1796.768554	124273.245870	37.458407
1799.077865	124454.765942	37.463424
1800.458243	124647.011626	37.468442
1802.549892	124840.086305	37.473460
1804.330442	125025.433673	37.478477
1806.471808	125211.004834	37.483495
1808.249236	125398.358834	37.488512
1810.196130	125588.326098	37.493530
1812.297583	125773.652325	37.498548
1813.747388	125948.411459	37.503565
1815.641515	126143.121601	37.508583
1818.161706	126327.662048	37.513600
1819.688128	126511.850529	37.518618
1821.416817	126699.471840	37.523636
1823.389783	126893.627757	37.528653
1824.969463	127084.800954	37.533671
1826.996117	127263.510349	37.538688
1828.165857	127461.295547	37.543706
1830.365487	127656.371306	37.548724
1832.026370	127843.957635	37.553741
1833.663721	128048.879134	37.558759
1836.032854	128254.398235	37.563776
1837.034438	128451.795645	37.568794
1839.138172	128649.974004	37.573812
1841.441972	128853.463562	37.578829
1842.723567	129055.438455	37.583847
1845.106309	129248.196734	37.588864
1846.759402	129453.351039	37.593882
1848.852901	129658.843802	37.598900
1850.743427	129866.640256	37.603917
1852.279176	130067.641548	37.608935
1854.484122	130269.465852	37.613952
1855.721948	130471.175187	37.618970
1857.603990	130688.746658	37.623988
1859.792529	130888.571749	37.629005
1861.526118	131103.364382	37.634023
1863.368063	131306.785341	37.639040
1865.321615	131513.044736	37.644058
1867.192650	131718.746989	37.649076
1869.097540	131925.789915	37.654093
1870.780623	132129.188722	37.659111
1872.852744	132333.543008	37.664128
1874.616044	132557.308973	37.669146
1876.267348	132764.408051	37.674164
1878.239466	132967.879988	37.679181
1880.390289	133171.578832	37.684199
1882.038064	133379.797974	37.689216
1883.876805	133588.737019	37.694234
1885.702475	133799.265197	37.699252
1887.639010	133994.296641	37.704269
1889.194089	134188.741174	37.709287
1890.976631	134378.646552	37.714304
1892.802592	134574.497164	37.719322
1894.366886	134774.754426	37.724340
1896.109200	134983.093277	37.729357
1898.039178	135181.100214	37.734375
1899.809734	135384.360834	37.739392
1901.830185	135593.471348	37.744410
1903.818457	135800.544843	37.749428
1906.019188	136014.159377	37.754445
1907.784963	136231.877890	37.759463
1909.587695	136427.054951	37.764480
1911.349011	136641.679858	37.769498
1913.424429	136853.706256	37.774516
1915.937475	137064.180822	37.779533
1917.787929	137268.909463	37.784551
1919.978932	137479.436057	37.789568
1921.853518	137701.560721	37.794586
1923.873584	137905.872409	37.799604
1925.982628	138112.188872	37.804621
1927.930341	138329.267212	37.809639
1930.390975	138522.840654	37.814656
1932.319429	138727.182906	37.819674
1933.809515	138940.172917	37.824692
1935.932990	139151.072934	37.829709
1937.841326	139356.931219	37.834727
1940.213001	139563.847745	37.839744
1942.210534	139767.879208	37.844762
1944.491203	139967.489240	37.849780
1947.114482	140167.592488	37.854797
1948.848116	140378.304851	37.859815
1950.404038	140569.057897	37.864832
1952.225877	140768.260454	37.869850
1954.216553	140978.922774	37.874868
1956.147034	141187.031828	37.879885
1957.747873	141396.386036	37.884903
1960.252714	141600.270238	37.889920
1962.044474	141813.644973	37.894938
1963.893460	142029.549967	37.899956
1965.653217	142245.292131	37.904973
1967.147028	142467.764920	37.909991
1969.271662	142678.819916	37.915008
1971.051695	142902.874625	37.920026
1972.568068	143129.941178	37.925044
1974.645110	143362.937274	37.930061
1976.083677	143588.152403	37.935079
1978.433791	143817.567209	37.940096
1979.862372	144065.402460	37.945114
1981.842019	144308.203415	37.950132
1983.854527	144559.123167	37.955149
1985.696636	144806.047386	37.960167
1987.682068	145042.149714	37.965184
1990.224413	145292.229156	37.970202
1991.678081	145543.164640	37.975220
1993.662667	145785.400816	37.980237
1995.495210	146040.430100	37.985255
1997.813182	146288.429783	37.990272
1999.878328	146526.785822	37.995290
2001.618328	146781.427050	38.000308
2003.831632	147018.353463	38.005325
2005.507807	147280.724057	38.010343
2007.663720	147536.700447	38.015360
2009.812071	147788.858811	38.020378
2011.877221	148045.600690	38.025396
2013.937836	148303.258409	38.030413
2015.623235	148556.863336	38.035431
2017.381344	148803.642125	38.040448
2019.390085	149039.556041	38.045466
2021.026953	149287.155604	38.050484
2023.001329	149518.926410	38.055501
2025.031588	149763.293717	38.060519
2027.076459	150009.132265	38.065536
2029.430758	150253.032501	38.070554
2031.436947	150496.036028	38.075572
2033.657202	150730.985185	38.080589
2035.362591	150981.666364	38.085607
2037.662667	151216.795601	38.090624
2039.725469	151466.763331	38.095642
2042.025734	151722.343853	38.100660
2043.891976	151957.988066	38.105677
2045.765077	152207.150915	38.110695
2048.059046	152464.677983	38.115712
2049.738177	152726.262379	38.120730
2051.710224	152985.314433	38.125748
2054.076578	153235.509485	38.130765
2055.815677	153498.154443	38.135783
2057.835987	153758.814685	38.140800
2060.288896	154025.590792	38.145818
2062.126743	154296.373657	38.150836
2063.918575	154559.053413	38.155853
2066.133611	154825.502161	38.160871
2068.070758	155097.707813	38.165888
2070.378815	155374.236569	38.170906
2072.242491	155650.124922	38.175924
2074.370721	155920.692525	38.180941
2076.443945	156204.599174	38.185959
2078.373222	156477.218747	38.190976
2081.126003	156754.916217	38.195994
2083.098189	157042.854145	38.201012
2085.183395	157318.538149	38.206029
2087.438225	157597.878526	38.211047
2089.469529	157872.646763	38.216064
2091.707585	158148.501236	38.221082
2093.623333	158438.130407	38.226100
2095.915222	158705.308379	38.231117
2098.100488	158982.393599	38.236135
2100.519925	159267.505058	38.241152
2102.935123	159546.042385	38.246170
2104.800208	159811.996713	38.251188
2107.200762	160086.679406	38.256205
2109.234933	160367.806113	38.261223
2111.293455	160638.710474	38.266240
2113.332672	160908.539898	38.271258
2115.448529	161203.927386	38.276276
2117.658049	161465.353634	38.281293
2120.140543	161747.076920	38.286311
2122.082320	162028.860215	38.291328
2124.675547	162289.201784	38.296346
2126.640721	162577.407912	38.301364
2128.822453	162839.821694	38.306381
2130.869673	163122.532871	38.311399
2132.714577	163384.925105	38.316416
2135.481459	163657.598350	38.321434
2137.366538	163934.752027	38.326452
2139.310436	164200.560065	38.331469
2141.239366	164477.341009	38.336487
2143.571519	164762.338305	38.341504
2146.059676	165015.711459	38.346522
2147.658063	165301.053781	38.351540
2149.831955	165566.679114	38.356557
2152.115134	165840.122191	38.361575
2153.877244	166122.090635	38.366592
2156.283882	166397.954468	38.371610
2158.105669	166687.216473	38.376628
2160.231149	166951.851702	38.381645
2162.066331	167216.126827	38.386663
2164.285977	167481.295381	38.391680
2166.326367	167744.753377	38.396698
2168.189927	168014.601003	38.401716
2170.162186	168272.281818	38.406733
2172.407864	168549.080704	38.411751
2174.117106	168832.630072	38.416768
2176.377008	169101.378995	38.421786
2177.947916	169391.668839	38.426804
2180.121980	169673.638234	38.431821
2182.076822	169969.863696	38.436839
2183.945731	170266.916358	38.441856
2186.672844	170573.105688	38.446874
2189.022703	170882.148420	38.451892
2191.037425	171174.153894	38.456909
2193.174156	171471.906165	38.461927
2195.099209	171795.151057	38.466944
2197.188869	172107.210561	38.471962
2199.453350	172419.637769	38.476980
2201.266612	172742.358096	38.481997
2204.044736	173061.526632	38.487015
2206.235248	173384.229032	38.492032
2208.884473	173689.135228	38.497050
2211.248830	174004.740459	38.502068
2213.045156	174324.841536	38.507085
2215.771626	174640.075507	38.512103
2218.320666	174963.706335	38.517120
2221.115351	175270.564184	38.522138
2223.237605	175580.245247	38.527156
2225.604770	175892.327427	38.532173
2228.001660	176202.057004	38.537191
2230.176646	176516.190488	38.542208
2232.590877	176817.716603	38.547226
2234.976845	177137.368768	38.552244
2237.507609	177431.958364	38.557261
2239.800474	177737.862237	38.562279
2241.468920	178045.058050	38.567296
2243.964832	178350.754750	38.572314
2246.225730	178659.816143	38.577332
2249.012095	178981.546292	38.582349
2250.999787	179285.699968	38.587367
2252.955322	179606.672814	38.592384
2255.362923	179916.426956	38.597402
2257.365484	180231.604112	38.602420
2259.697331	180552.521814	38.607437
2262.157345	180869.992009	38.612455
2264.047503	181195.323758	38.617472
2266.475752	181509.880372	38.622490
2268.485125	181837.176889	38.627508
2270.678383	182157.207468	38.632525
2272.776460	182480.504933	38.637543
2275.380502	182811.953829	38.642560
2277.592682	183133.203905	38.647578
2279.749641	183465.969182	38.652596
2281.840905	183794.885246	38.657613
2284.071243	184120.605946	38.662631
2285.926757	184462.946063	38.667648
2288.589630	184795.967335	38.672666
2290.676205	185134.463987	38.677684
2292.903845	185473.143022	38.682701
2295.316285	185823.528823	38.687719
2297.218386	186239.779209	38.692736
2299.811637	186569.286666	38.697754
2302.151785	186907.089358	38.702772
2304.789214	187240.452767	38.707789
2307.557468	187569.453548	38.712807
2309.347518	187918.266887	38.717824
2311.683461	188234.459383	38.722842
2313.611579	188557.955205	38.727860
2315.883663	188872.279909	38.732877
2318.395131	189191.216439	38.737895
2319.816310	189510.196561	38.742912
2322.363471	189824.430346	38.747930
2324.749849	190151.186891	38.752948
2326.991722	190460.491518	38.757965
2329.484080	190795.031266	38.762983
2331.913428	191120.767861	38.768000
2334.244569	191448.425675	38.773018
2336.679618	191784.501186	38.778036
2338.503305	192108.556718	38.783053
2341.112906	192445.419729	38.788071
2343.390320	192782.182962	38.793088
2345.723620	193123.104142	38.798106
2347.805988	193466.554590	38.803124
2349.807249	193826.554586	38.808141
2352.741032	194169.569627	38.813159
2355.359050	194513.777770	38.818176
2357.675677	194862.402718	38.823194
2360.249948	195206.898905	38.828212
2362.461993	195549.471058	38.833229
2364.843058	195906.039301	38.838247
2366.911868	196274.011488	38.843264
2369.237427	196623.223835	38.848282
2371.449202	196991.201076	38.853300
2373.469283	197362.511312	38.858317
2375.776957	197738.578664	38.863335
2378.232574	198126.715179	38.868352
2380.226074	198505.500577	38.873370
2382.263524	198892.002256	38.878388
2384.503978	199284.239560	38.883405
2386.786752	199673.626260	38.888423
2389.058488	200080.822475	38.893440
2391.589184	200472.255538	38.898458
2394.381375	200874.444776	38.903476
2396.958516	201273.467792	38.908493
2399.677856	201676.203772	38.913511
2402.294732	202069.862622	38.918528
2404.841944	202465.387592	38.923546
2407.493458	202843.979192	38.928564
2410.219023	203236.734676	38.933581
2413.065422	203625.356995	38.938599
2415.149393	204016.003985	38.943616
2417.479970	204400.948619	38.948634
2420.298589	204787.824895	38.953652
2422.393996	205184.746977	38.958669
2425.218804	205566.746500	38.963687
2427.771689	205951.126130	38.968704
2430.045353	206327.802046	38.973722
2432.287699	206725.212329	38.978740
2434.997696	207119.121169	38.983757
2438.245980	207479.897581	38.988775
2440.574525	207858.676087	38.993792
2443.169577	208237.007300	38.998810
2445.562385	208611.534726	39.003828
2448.157543	209002.771973	39.008845
2450.424316	209363.018179	39.013863
2453.250577	209733.008913	39.018880
2455.478739	210105.709809	39.023898
2458.235836	210487.423330	39.028916
2460.353725	210867.077588	39.033933
2462.930545	211228.345077	39.038951
2465.158509	211604.706177	39.043968
2467.611091	211978.797308	39.048986
2470.156470	212346.472783	39.054004
2472.696437	212715.089480	39.059021
2475.199510	213072.331546	39.064039
2477.612847	213430.858159	39.069056
2479.538404	213778.969367	39.074074
2482.153029	214125.297056	39.079092
2484.244749	214481.258256	39.084109
2486.561166	214831.367389	39.089127
2489.410203	215202.326651	39.094144
2491.310703	215557.962991	39.099162
2493.648135	215912.947366	39.104180
2495.603059	216291.363083	39.109197
2498.020679	216660.460133	39.114215
2500.454919	217047.007354	39.119232
2502.651791	217433.668048	39.124250
2504.848691	217821.624645	39.129268
2507.187815	218221.600862	39.134285
2509.552855	218619.566434	39.139303
2512.280917	219018.542758	39.144320
2514.803284	219428.703702	39.149338
2518.019468	219826.131156	39.154356
2520.421639	220238.826307	39.159373
2522.966496	220637.984551	39.164391
2525.473930	221041.950183	39.169408
2527.788263	221453.948331	39.174426
2530.449537	221870.185955	39.179444
2532.871494	222289.509477	39.184461
2535.619894	222699.560674	39.189479
2538.035825	223134.534331	39.194496
2540.444709	223556.400704	39.199514
2543.273053	223988.998637	39.204532
2545.646490	224401.826853	39.209549
2548.436222	224832.169979	39.214567
2551.016936	225269.887463	39.219584
2553.560025	225693.765596	39.224602
2556.524552	226115.825268	39.229620
2558.857741	226553.657507	39.234637
2561.192147	226982.623494	39.239655
2564.164552	227429.857301	39.244672
2566.430970	227866.810627	39.249690
2568.933083	228300.780306	39.254708
2571.868297	228749.924916	39.259725
2573.957465	229178.826986	39.264743
2576.732003	229621.365842	39.269760
2579.469156	230082.480689	39.274778
2582.265255	230523.618576	39.279796
2584.865680	230967.454112	39.284813
2587.296118	231404.151927	39.289831
2589.715593	231855.915752	39.294848
2592.282625	232313.067360	39.299866
2594.820035	232758.537429	39.304884
2597.461914	233216.794486	39.309901
2599.893257	233671.933843	39.314919
2602.786437	234125.603718	39.319936
2605.653686	234581.004674	39.324954
2608.095606	235035.124973	39.329972
2610.780146	235492.433335	39.334989
2613.782641	235940.825803	39.340007
2616.680731	236398.963659	39.345024
2619.687023	236833.890535	39.350042
2622.462791	237271.875816	39.355060
2624.973839	237718.945459	39.360077
2627.613979	238150.371201	39.365095
2630.619121	238593.145794	39.370112
2632.742661	239033.465807	39.375130
2635.347990	239474.980394	39.380148
2637.690021	239919.228075	39.385165
2640.260954	240369.053614	39.390183
2642.805743	240813.217544	39.395200
2645.024870	241266.170186	39.400218
2648.328538	241691.847937	39.405236
2650.496268	242130.809850	39.410253
2652.995505	242543.376255	39.415271
2655.503241	242960.665634	39.420288
2658.098155	243391.607607	39.425306
2660.564358	243817.615209	39.430324
2663.114960	244253.312842	39.435341
2665.272310	244683.939411	39.440359
2668.053668	245127.702951	39.445376
2670.344770	245576.774849	39.450394
2673.262256	246021.277396	39.455412
2675.318855	246482.145312	39.460429
2678.308664	246936.338430	39.465447
2680.979102	247392.714006	39.470464
2683.483682	247862.984109	39.475482
2686.025422	248317.040424	39.480500
2688.883017	248789.996688	39.485517
2691.149442	249265.558530	39.490535
2694.692927	249746.839080	39.495552
2696.790213	250224.710810	39.500570
2699.504654	250709.699352	39.505588
2702.322517	251197.566207	39.510605
2705.069467	251674.875378	39.515623
2707.821520	252162.851130	39.520640
2710.325858	252662.929782	39.525658
2713.161367	253147.891999	39.530676
2715.994876	253654.266584	39.535693
2718.396768	254151.536611	39.540711
2721.636972	254639.148895	39.545728
2724.467795	255143.359542	39.550746
2727.702807	255632.036048	39.555764
2731.004235	256127.482609	39.560781
2734.238180	256610.719895	39.565799
2737.336792	257096.135571	39.570816
2739.841350	257579.254198	39.575834
2742.471247	258069.971766	39.580852
2745.308004	258567.284844	39.585869
2748.618117	259037.318157	39.590887
2751.192890	259523.288663	39.595904
2754.106147	260006.512096	39.600922
2757.188885	260483.611112	39.605940
2759.738357	260970.163880	39.610957
2762.627439	261448.279708	39.615975
2765.497642	261912.248651	39.620992
2768.126861	262398.122548	39.626010
2770.394106	262880.088286	39.631028
2773.202423	263371.010017	39.636045
2775.741301	263862.733450	39.641063
2778.578074	264354.103479	39.646080
2781.170205	264853.865693	39.651098
2783.839528	265363.112825	39.656116
2786.588299	265865.207930	39.661133
2789.083252	266362.819040	39.666151
2792.043782	266865.358818	39.671168
2794.235281	267397.148080	39.676186
2797.250727	267896.626221	39.681204
2799.714468	268411.020352	39.686221
2802.956388	268922.293620	39.691239
2805.851548	269430.341725	39.696256
2808.554006	269940.779079	39.701274
2811.636292	270450.925929	39.706292
2814.625265	270960.576499	39.711309
2817.193809	271475.597728	39.716327
2820.700907	271979.802992	39.721344
2823.542020	272488.147198	39.726362
2826.261909	272979.846757	39.731380
2829.087574	273496.720930	39.736397
2832.058393	274001.632858	39.741415
2834.641908	274493.268759	39.746432
2837.198856	274979.166284	39.751450
2839.992191	275454.408465	39.756468
2842.563497	275941.212371	39.761485
2844.953781	276413.895885	39.766503
2847.877535	276892.944195	39.771520
2850.168892	277386.766842	39.776538
2852.774447	277889.451398	39.781556
2855.701157	278379.308808	39.786573
2858.896919	278879.076238	39.791591
2861.664934	279383.071796	39.796608
2864.753445	279898.137162	39.801626
2867.308125	280396.343726	39.806644
2870.369603	280901.502430	39.811661
2872.840378	281415.079008	39.816679
2875.636580	281933.350090	39.821696
2878.434662	282457.483230	39.826714
2881.386559	282991.416079	39.831732
2884.123068	283517.480994	39.836749
2886.750344	284048.790070	39.841767
2890.050297	284584.027985	39.846784
2892.421424	285133.550311	39.851802
2895.385281	285681.300074	39.856820
2898.470902	286234.485930	39.861837
2901.341693	286791.661925	39.866855
2904.370381	287348.783317	39.871872
2906.979090	287903.934015	39.876890
2909.714172	288467.439687	39.881908
2912.834520	289027.097169	39.886925
2915.331656	289614.853561	39.891943
2918.876627	290177.938961	39.896960
2921.954313	290745.180026	39.901978
2924.936122	291322.155555	39.906996
2927.873189	291900.249885	39.912013
2930.889913	292468.297240	39.917031
2934.107267	293041.944696	39.922048
2936.822880	293621.783752	39.927066
2939.731317	294192.472359	39.932084
2942.868894	294777.667933	39.937101
2945.519549	295355.849940	39.942119
2948.782470	295929.944925	39.947136
2951.856532	296526.253242	39.952154
2954.986429	297110.741146	39.957172
2958.299748	297694.534446	39.962189
2961.475733	298277.276823	39.967207
2964.592174	298834.355644	39.972224
2967.444345	299425.641299	39.977242
2970.411564	299997.710173	39.982260
2974.083155	300580.300524	39.987277
2977.047547	301145.224179	39.992295
2980.026833	301707.347139	39.997312
2983.271054	302281.887483	40.002330
2986.277188	302848.639904	40.007348
2989.481209	303419.645593	40.012365
2992.760028	303984.312544	40.017383
2995.560827	304531.735310	40.022400
2998.747999	305103.791349	40.027418
3001.940281	305660.533506	40.032436
3004.870719	306219.645669	40.037453
3007.806919	306786.416654	40.042471
3010.875800	307335.189137	40.047488
3013.573471	307902.010025	40.052506
3016.688757	308453.605883	40.057524
3019.931512	309004.591937	40.062541
3023.153525	309559.864632	40.067559
3026.157089	310115.698008	40.072576
3029.512928	310670.784868	40.077594
3032.060413	311225.280425	40.082612
3035.253382	311765.303372	40.087629
3037.819715	312292.676495	40.092647
3040.570703	312806.588659	40.097664
3043.521822	313339.448501	40.102682
3046.417343	313870.788098	40.107700
3049.198986	314390.464649	40.112717
3051.821847	314930.133642	40.117735
3054.657499	315466.920693	40.122752
3057.387361	316020.112578	40.127770
3060.290950	316564.388182	40.132788
3063.468011	317118.968932	40.137805
3065.850088	317684.122182	40.142823
3069.210977	318248.760629	40.147840
3072.109121	318818.184014	40.152858
3074.706859	319405.283673	40.157876
3078.106323	319977.278502	40.162893
3081.034275	320561.139073	40.167911
3084.123694	321151.107545	40.172928
3087.508033	321751.958812	40.177946
3090.788124	322349.645908	40.182964
3093.980761	322940.080963	40.187981
3097.001992	323531.447857	40.192999
3100.335285	324130.699879	40.198016
3103.408972	324735.413597	40.203034
3106.551863	325338.103174	40.208052
3109.534239	325941.620787	40.213069
3112.494781	326551.577472	40.218087
3115.820304	327162.584533	40.223104
3119.325639	327774.340847	40.228122
3122.607803	328375.948590	40.233140
3126.502790	328969.992776	40.238157
3129.496115	329586.113919	40.243175
3133.126894	330180.155578	40.248192
3136.358178	330784.169964	40.253210
3139.956126	331372.946956	40.258228
3143.336050	331966.416793	40.263245
3146.707020	332565.764369	40.268263
3149.856003	333153.391561	40.273280
3152.582061	333746.529555	40.278298
3155.831938	334352.235075	40.283316
3159.030311	334942.109782	40.288333
3161.776093	335553.378947	40.293351
3165.056352	336156.818167	40.298368
3168.642808	336763.598886	40.303386
3171.215218	337368.498133	40.308404
3174.285133	337963.138578	40.313421
3177.444787	338597.222560	40.318439
3180.809748	339196.793631	40.323456
3183.620866	339813.510633	40.328474
3186.616322	340437.645087	40.333492
3190.329852	341054.225529	40.338509
3192.950632	341681.972506	40.343527
3196.340814	342298.530749	40.348544
3199.476444	342923.233382	40.353562
3202.600601	343551.882881	40.358580
3206.303253	344176.956529	40.363597
3209.118498	344804.439304	40.368615
3212.411148	345420.373735	40.373632
3216.162070	346050.908637	40.378650
3219.422273	346674.661308	40.383668
3222.588318	347283.607882	40.388685
3225.980743	347905.440599	40.393703
3229.327490	348533.633485	40.398720
3232.632287	349140.749507	40.403738
3235.851547	349767.924503	40.408756
3239.513495	350379.298009	40.413773
3241.980977	351005.830948	40.418791
3244.901850	351628.148411	40.423808
3248.923454	352225.029642	40.428826
3251.723505	352824.270319	40.433844
3254.822786	353398.454715	40.438861
3257.774671	353986.950788	40.443879
3260.458441	354571.446615	40.448896
3263.733012	355157.588976	40.453914
3266.557200	355764.604126	40.458932
3269.984178	356358.888861	40.463949
3273.413412	356967.028669	40.468967
3276.108302	357574.915914	40.473984
3279.851600	358198.040576	40.479002
3282.170545	358810.854376	40.484020
3285.868154	359430.031974	40.489037
3288.866997	360065.477739	40.494055
3291.973857	360701.324262	40.499072
3295.366839	361331.511163	40.504090
3298.517728	361976.828952	40.509108
3302.018536	362621.850220	40.514125
3304.873944	363276.208943	40.519143
3307.969751	363940.780387	40.524160
3311.337342	364609.298898	40.529178
3314.584683	365268.190291	40.534196
3318.270739	365935.209642	40.539213
3321.799382	366618.279879	40.544231
3324.542997	367290.026946	40.549248
3328.652558	367968.109112	40.554266
3332.019807	368649.356903	40.559284
3335.036356	369340.398839	40.564301
3338.437614	370023.382131	40.569319
3341.518396	370708.704553	40.574336
3345.369466	371405.672577	40.579354
3348.640509	372100.914476	40.584372
3351.856676	372797.389003	40.589389
3355.275527	373494.473168	40.594407
3358.882587	374205.495597	40.599424
3362.464104	374892.131335	40.604442
3366.509526	375562.818299	40.609460
3370.225778	376260.140220	40.614477
3373.892087	376950.586642	40.619495
3377.725570	377644.941137	40.624512
3380.975312	378323.080152	40.629530
3384.493953	379011.140468	40.634548
3388.053228	379695.427686	40.639565
3391.578139	380385.123049	40.644583
3394.909924	381056.998681	40.649600
3398.218124	381742.259434	40.654618
3401.015546	382430.392997	40.659636
3404.575363	383109.879749	40.664653
3407.958639	383804.419939	40.669671
3411.072709	384513.292242	40.674688
3415.156738	385209.686002	40.679706
3418.503213	385899.971012	40.684724
3422.256070	386585.261189	40.689741
3425.556045	387274.908111	40.694759
3429.391707	387940.928373	40.699776
3433.317280	388619.425753	40.704794
3436.258790	389313.452854	40.709812
3439.925770	389987.749838	40.714829
3443.720559	390666.540697	40.719847
3446.830191	391342.887553	40.724864
3450.492036	392030.472286	40.729882
3453.886363	392702.838208	40.734900
3457.182474	393370.896960	40.739917
3461.012261	394059.512024	40.744935
3463.890569	394733.876408	40.749952
3467.277805	395405.256783	40.754970
3471.067712	396092.300807	40.759988
3474.451474	396775.236845	40.765005
3477.978426	397430.056088	40.770010
3481.365386	398044.814242	40.775015
3484.508260	398632.594464	40.780020
3487.534248	399176.123797	40.785024
3490.410304	399664.753062	40.790029
3493.364447	400104.540005	40.795034
3495.810151	400501.922086	40.800039
3497.768970	400843.399475	40.805044
3500.435246	401158.982729	40.810048
3501.817343	401410.619220	40.815053
3503.935550	401637.476338	40.820058
3505.585701	401819.545832	40.825063
3506.940088	401971.467064	40.830068
3508.172390	402092.909141	40.835072
3509.328145	402177.370247	40.840077
3510.746312	402242.761325	40.845082
3511.467044	402286.085797	40.850087
3512.762041	402281.317407	40.855092
3513.629716	402276.666258	40.860096
3514.323284	402227.844445	40.865101
3514.625494	402167.361598	40.870106
3515.002353	402104.076055	40.875111
3515.950871	402007.514682	40.880116
3516.162055	401913.706354	40.885120
3516.214616	401798.812548	40.890125
3516.596747	401666.562854	40.895130
3517.133887	401536.470326	40.900135
3517.577431	401391.269453	40.905140
3517.316256	401238.514698	40.910144
3517.599052	401072.987718	40.915149
3517.545888	400914.920842	40.920154
3517.373375	400746.163846	40.925159
3517.522430	400564.719483	40.930164
3517.509528	400390.657332	40.935168
3517.559551	400218.055782	40.940173
3517.407185	400027.316464	40.945178
3517.205129	399844.398658	40.950183
3517.283016	399649.205252	40.955188
3516.866316	399463.069893	40.960192
3516.840263	399275.197502	40.965197
3516.797311	399082.758677	40.970202
3516.598067	398902.066076	40.975207
3516.809853	398708.518763	40.980212
3516.688734	398522.431427	40.985216
3516.102309	398328.700682	40.990221
3515.839462	398128.726159	40.995226
3515.828607	397947.083344	41.000231
3515.608718	397770.191729	41.005236
3515.311207	397567.172625	41.010240
3515.332865	397392.879796	41.015245
3515.334612	397202.601062	41.020250
3514.595584	397021.978026	41.025255
3514.770365	396837.912307	41.030260
3514.251006	396669.636729	41.035264
3514.047245	396504.965291	41.040269
3514.014820	396331.586682	41.045274
3513.922963	396161.972070	41.050279
3513.593963	395977.470511	41.055284
3512.948303	395810.680468	41.060288
3512.841555	395647.307699	41.065293
3513.103040	395489.510687	41.070298
3512.598346	395327.669649	41.075303
3512.594679	395169.150403	41.080308
3512.258236	395011.747839	41.085312
3511.846782	394865.726079	41.090317
3511.717841	394719.710227	41.095322
3511.243631	394578.874003	41.100327
3511.490263	394429.853850	41.105332
3511.291110	394300.445079	41.110336
3511.006063	394156.226726	41.115341
3511.348108	394012.569826	41.120346
3510.973105	393886.079596	41.125351
3510.831645	393748.537007	41.130356
3510.846819	393606.400654	41.135360
3510.782919	393468.945929	41.140365
3510.590606	393337.195848	41.145370
3510.079360	393209.403443	41.150375
3510.152793	393074.564792	41.155380
3509.697447	392958.793294	41.160384
3509.523108	392820.742913	41.165389
3509.628426	392701.481757	41.170394
3509.422553	392580.288627	41.175399
3509.511398	392469.557324	41.180404
3509.610317	392352.630629	41.185408
3509.051929	392238.039326	41.190413
3508.653036	392121.848936	41.195418
3508.728186	392015.838886	41.200423
3508.691455	391908.627405	41.205428
3508.737442	391797.290528	41.210432
3508.202991	391678.428520	41.215437
3508.491916	391578.221432	41.220442
3508.346900	391500.114221	41.225447
3508.129951	391383.638174	41.230452
3508.374721	391280.187655	41.235456
3508.328466	391180.691074	41.240461
3507.886521	391070.391402	41.245466
3507.458416	390982.985356	41.250471
3507.462983	390881.245870	41.255476
3507.555915	390796.347248	41.260480
3507.336669	390691.443411	41.265485
3507.645349	390607.525931	41.270490
3507.323965	390520.304707	41.275495
3507.221076	390426.829982	41.280500
3507.107027	390345.211223	41.285504
3507.034351	390261.935755	41.290509
3506.957566	390162.465192	41.295514
3506.556001	390085.637261	41.300519
3506.919140	390006.151603	41.305524
3506.854065	389929.473903	41.310528
3506.816888	389846.699210	41.315533
3506.880037	389755.099984	41.320538
3506.339902	389683.369394	41.325543
3506.649713	389599.803709	41.330548
3506.587630	389516.270228	41.335552
3506.262865	389434.072002	41.340557
3506.485443	389354.073031	41.345562
3506.128519	389282.135070	41.350567
3506.008865	389202.138094	41.355572
3506.177484	389140.246839	41.360576
3505.837474	389060.639098	41.365581
3506.098858	388985.862389	41.370586
3505.877043	388916.618640	41.375591
3505.672848	388832.191077	41.380596
3505.566086	388763.030541	41.385600
3505.748558	388706.568691	41.390605
3505.715973	388628.561832	41.395610
3505.616876	388571.102653	41.400615
3505.639504	388502.124349	41.405620
3505.565358	388433.998668	41.410624
3505.578408	388370.225722	41.415629
3505.702305	388294.021299	41.420634
3505.255133	388244.764644	41.425639
3505.664413	388173.262755	41.430644
3505.604579	388107.901115	41.435648
3505.471606	388045.825595	41.440653
3505.607013	387973.629534	41.445658
3505.336244	387915.103920	41.450663
3505.234125	387850.611347	41.455668
3504.910968	387780.897861	41.460672
3504.948080	387723.060117	41.465677
3505.176236	387652.828901	41.470682
3504.975164	387597.033526	41.475687
3504.873737	387542.491891	41.480692
3504.867622	387482.172352	41.485696
3504.646449	387427.344451	41.490701
3504.781479	387376.827663	41.495706
3504.630958	387321.074583	41.500711
3504.601000	387264.845640	41.505716
3504.754189	387212.015416	41.510720
3504.374761	387158.937922	41.515725
3504.867053	387096.661202	41.520730
3504.959967	387052.776547	41.525735
3504.919345	386992.588142	41.530740
3504.647403	386934.669736	41.535744
3504.309453	386877.980095	41.540749
3504.364722	386824.808864	41.545754
3504.573101	386781.921294	41.550759
3504.743359	386734.190434	41.555764
3504.381349	386679.408207	41.560768
3504.392733	386640.765506	41.565773
3504.638401	386569.513010	41.570778
3504.469364	386523.764068	41.575783
3504.471599	386473.773904	41.580788
3504.298221	386411.421361	41.585792
3504.031095	386367.413821	41.590797
3504.276669	386318.147140	41.595802
3504.341654	386271.701220	41.600807
3504.149150	386225.803058	41.605812
3504.080928	386171.989562	41.610816
3503.956757	386128.060914	41.615821
3504.225997	386080.288029	41.620826
3503.888757	386034.386653	41.625831
3504.183467	385987.117407	41.630836
3503.952613	385942.062534	41.635840
3504.270723	385896.820600	41.640845
3503.552021	385843.945468	41.645850
3503.434930	385812.887450	41.650855
3503.902435	385766.174853	41.655860
3503.786391	385721.685674	41.660864
3503.822538	385675.370095	41.665869
3503.972724	385637.262827	41.670874
3503.673283	385605.572808	41.675879
3503.709103	385552.935108	41.680884
3503.812756	385512.854521	41.685888
3503.609443	385469.394058	41.690893
3503.926465	385429.813317	41.695898
3503.688375	385386.155007	41.700903
3503.785218	385343.130022	41.705908
3504.036935	385309.475035	41.710912
3503.699062	385262.226710	41.715917
3503.749127	385216.847549	41.720922
3503.398577	385173.155594	41.725927
3503.188511	385140.587835	41.730932
3503.239296	385103.358489	41.735936
3503.393503	385064.183364	41.740941
3503.453682	385033.452266	41.745946
3503.378654	385002.843730	41.750951
3503.761280	384958.478737	41.755956
3503.165030	384923.152505	41.760960
3503.054136	384887.547575	41.765965
3503.829378	384857.492085	41.770970
3503.532291	384816.736450	41.775975
3503.782759	384782.090747	41.780980
3503.671677	384732.038618	41.785984
3503.562874	384693.995632	41.790989
3503.826294	384654.371249	41.795994
3503.364345	384612.015963	41.800999
3503.381263	384574.511823	41.806004
3503.291132	384541.848464	41.811008
3503.398481	384502.222742	41.816013
3503.686520	384459.572762	41.821018
3503.495540	384422.837076	41.826023
3503.312475	384384.221203	41.831028
3503.070507	384351.809744	41.836032
3503.269367	384315.749567	41.841037
3503.389547	384277.492595	41.846042
3503.445243	384242.647955	41.851047
3503.288609	384206.973023	41.856052
3503.433627	384171.352664	41.861056
3503.500613	384134.855720	41.866061
3503.893347	384083.352818	41.871066
3503.608837	384044.472920	41.876071
3503.672830	384012.216548	41.881076
3503.593061	383971.908177	41.886080
3503.404387	383927.071698	41.891085
3503.373258	383887.136491	41.896090
3503.390934	383844.629126	41.901095
3503.158013	383821.153255	41.906100
3503.247412	383792.142717	41.911104
3503.156003	383760.291078	41.916109
3503.400409	383715.970835	41.921114
3502.824616	383688.561774	41.926119
3503.302525	383650.679853	41.931124
3503.320909	383621.578608	41.936128
3503.234215	383583.784447	41.941133
3503.689559	383549.181372	41.946138
3503.361300	383515.842804	41.951143
3503.593050	383474.164823	41.956148
3503.440479	383430.362909	41.961152
3503.299627	383404.104655	41.966157
3503.357694	383361.031592	41.971162
3503.475927	383325.795104	41.976167
3503.581860	383292.490248	41.981172
3503.141746	383249.189821	41.986176
3502.984179	383224.102002	41.991181
3503.530241	383180.698783	41.996186
3503.194570	383149.976245	42.001191
3503.317823	383105.572239	42.006196
3503.121181	383069.698820	42.011200
3502.909912	383044.771535	42.016205
3502.901036	383003.054061	42.021210
3502.673098	382980.947812	42.026215
3503.069591	382942.848994	42.031220
3503.239952	382915.830838	42.036224
3503.094901	382880.533145	42.041229
3503.399198	382842.854800	42.046234
3503.054144	382812.590377	42.051239
3503.218799	382772.572193	42.056244
3503.195562	382741.267314	42.061248
3503.113496	382708.168704	42.066253
3503.187894	382669.053133	42.071258
3502.900483	382634.234317	42.076263
3503.434312	382603.959846	42.081268
3503.435613	382576.764506	42.086272
3503.000434	382548.011948	42.091277
3503.222308	382503.413815	42.096282
3503.148133	382468.485417	42.101287
3502.942879	382443.734362	42.106292
3503.501029	382397.077712	42.111296
3503.486842	382370.341631	42.116301
3503.357855	382329.073436	42.121306
3502.903531	382308.093722	42.126311
3503.316993	382263.084473	42.131316
3503.187461	382235.985313	42.136320
3503.160300	382204.680397	42.141325
3503.177634	382157.625013	42.146330
3502.938737	382128.663695	42.151335
3502.995984	382090.717988	42.156340
3503.240573	382057.364574	42.161344
3503.258623	382025.442978	42.166349
3503.226518	381995.306651	42.171354
3502.774075	381975.799164	42.176359
3502.751532	381931.771336	42.181364
3503.096414	381899.240080	42.186368
3502.617235	381872.169557	42.191373
3503.192998	381845.214167	42.196378
3502.951029	381814.551641	42.201383
3503.049385	381778.960640	42.206388
3502.733667	381742.342120	42.211392
3502.758304	381722.531664	42.216397
3503.189104	381682.952856	42.221402
3502.792547	381648.454420	42.226407
3502.803440	381616.025570	42.231412
3502.818777	381585.170375	42.236416
3503.036517	381554.943873	42.241421
3502.527184	381523.662383	42.246426
3502.398618	381502.478964	42.251431
3502.673430	381481.918380	42.256436
3502.665740	381443.931049	42.261440
3502.894410	381432.823970	42.266445
3502.986654	381395.506641	42.271450
3503.279134	381374.486140	42.276455
3503.018231	381337.223682	42.281460
3503.235954	381306.158908	42.286464
3502.876117	381265.356640	42.291469
3503.013230	381238.570459	42.296474
3502.827651	381206.730335	42.301479
3502.663173	381171.052437	42.306484
3502.465853	381145.257769	42.311488
3502.634741	381121.183654	42.316493
3502.602722	381084.774000	42.321498
3502.543118	381066.042695	42.326503
3502.692637	381032.753553	42.331508
3503.097866	381005.950805	42.336512
3502.609322	380972.329181	42.341517
3502.748906	380937.111526	42.346522
3502.482794	380917.244128	42.351527
3502.661605	380892.508015	42.356532
3502.831099	380874.198014	42.361536
3502.487395	380851.701663	42.366541
3502.600803	380813.034326	42.371546
3502.954286	380795.559038	42.376551
3502.565832	380763.165879	42.381556
3502.738975	380741.046099	42.386560
3502.476393	380719.349623	42.391565
3502.443134	380688.907239	42.396570
3502.431505	380665.774987	42.401575
3502.585240	380634.516220	42.406580
3502.589107	380615.266830	42.411584
3502.290433	380589.030290	42.416589
3502.391054	380565.474173	42.421594
3502.299153	380539.840265	42.426599
3502.012458	380524.521356	42.431604
3502.467329	380496.085125	42.436608
3502.538249	380482.234205	42.441613
3502.729948	380450.029719	42.446618
3502.590487	380424.479282	42.451623
3502.503658	380402.653617	42.456628
3502.659467	380362.887057	42.461632
3502.610064	380348.165983	42.466637
3502.618545	380317.945223	42.471642
3502.473286	380297.017372	42.476647
3502.662187	380266.920846	42.481652
3502.875884	380233.442941	42.486656
3502.421958	380209.058593	42.491661
3502.878002	380181.764600	42.496666
3502.319648	380160.469212	42.501671
3502.187371	380135.374481	42.506676
3502.220910	380118.684977	42.511680
3502.309887	380100.107624	42.516685
3502.654417	380076.995615	42.521690
3502.238426	380056.084306	42.526695
3502.508691	380028.920644	42.531700
3502.585045	379993.736959	42.536704
3502.534551	379981.199807	42.541709
3502.898124	379937.438673	42.546714
3502.507174	379918.758111	42.551719
3502.486136	379893.518864	42.556724
3502.509377	379879.116357	42.561728
3502.449545	379847.762915	42.566733
3502.735399	379819.936341	42.571738
3502.676600	379792.620482	42.576743
3502.763605	379761.421852	42.581748
3502.598079	379736.560471	42.586752
3502.457162	379709.562045	42.591757
3502.405250	379674.575660	42.596762
3502.577478	379662.130673	42.601767
3502.716238	379628.562082	42.606772
3502.376781	379606.292559	42.611776
3502.712367	379571.423505	42.616781
3502.857234	379549.180148	42.621786
3502.856162	379526.730925	42.626791
3503.116083	379494.971772	42.631796
3502.907957	379459.399923	42.636800
3502.625686	379430.874091	42.641805
3502.630163	379405.173289	42.646810
3502.511271	379389.929189	42.651815
3502.459794	379375.868175	42.656820
3502.483980	379336.907811	42.661824
3502.165112	379308.336750	42.666829
3502.584448	379276.857274	42.671834
3502.692198	379263.457103	42.676839
3502.555282	379233.689452	42.681844
3502.714321	379198.796589	42.686848
3502.538929	379172.742617	42.691853
3502.631724	379145.656456	42.696858
3502.730230	379127.203915	42.701863
3502.379002	379094.472764	42.706868
3502.482637	379070.991032	42.711872
3502.456486	379049.002430	42.716877
3502.248980	379011.322033	42.721882
3502.173690	378999.550147	42.726887
3502.336462	378970.268877	42.731892
3502.738406	378945.673988	42.736896
3502.597054	378921.290599	42.741901
3502.822434	378895.834283	42.746906
3502.356946	378877.139185	42.751911
3502.987661	378857.105278	42.756916
3502.813387	378820.968592	42.761920
3502.726710	378796.221036	42.766925
3502.505410	378756.485347	42.771930
3502.170276	378742.137989	42.776935
3502.196167	378721.563196	42.781940
3502.461856	378694.830611	42.786945
3502.294096	378674.438293	42.791949
3502.819816	378649.036589	42.796954
3502.622760	378624.458427	42.801959
3502.408474	378592.492628	42.806964
3502.678573	378560.426019	42.811969
3502.590259	378541.570406	42.816973
3502.641260	378516.115466	42.821978
3502.811283	378488.026161	42.826983
3502.678262	378465.291817	42.831988
3502.550139	378434.506048	42.836993
3502.315111	378406.530481	42.841997
3502.388338	378387.192486	42.847002
3502.207131	378359.691026	42.852007
3502.222174	378339.016040	42.857012
3502.675791	378311.339555	42.862017
3502.579147	378293.450128	42.867021
3502.724019	378269.453342	42.872026
3502.831985	378232.078299	42.877031
3502.735908	378209.566556	42.882036
3502.537931	378185.089717	42.887041
3502.492724	378157.617678	42.892045
3502.758964	378120.192453	42.897050
3502.425925	378106.885688	42.902055
3502.181472	378081.196946	42.907060
3502.417451	378036.284286	42.912065
3502.575533	378023.358197	42.917069
3502.559779	377998.014737	42.922074
3502.172950	377979.814702	42.927079
3502.506203	377960.943871	42.932084
3502.577120	377922.685272	42.937089
3502.591473	377902.517992	42.942093
3502.646122	377878.484100	42.947098
3502.345787	377852.956215	42.952103
3502.680301	377840.281947	42.957108
3502.468229	377799.527517	42.962113
3502.014523	377777.325030	42.967117
3502.816966	377750.380989	42.972122
3502.771763	377726.387895	42.977127
3502.469194	377694.866507	42.982132
3502.658980	377675.205095	42.987137
3502.781697	377649.306418	42.992141
3502.425680	377630.517216	42.997146
3502.476710	377608.490017	43.002151
3502.578302	377578.632605	43.007156
3502.382252	377541.583274	43.012161
3502.231190	377537.492487	43.017165
3502.463974	377505.074857	43.022170
3502.392355	377475.498256	43.027175
3502.381485	377449.975736	43.032180
3502.500224	377423.315541	43.037185
3502.207029	377413.151497	43.042189
3502.287144	377378.293930	43.047194
3502.323101	377362.872187	43.052199
3502.213772	377341.580849	43.057204
3502.457298	377311.218501	43.062209
3502.233183	377301.526216	43.067213
3502.460210	377271.902917	43.072218
3502.134411	377249.349920	43.077223
3502.394111	377222.388218	43.082228
3502.296443	377204.802993	43.087233
3502.107601	377183.854070	43.092237
3502.548743	377161.943581	43.097242
3502.504942	377138.635477	43.102247
3502.250064	377102.407416	43.107252
3502.531452	377081.766204	43.112257
3502.325958	377064.477040	43.117261
3502.109722	377042.516363	43.122266
3502.682588	377024.826676	43.127271
3502.565585	377002.317174	43.132276
3502.828617	376964.332084	43.137281
3502.046201	376950.866092	43.142285
3502.440156	376916.086076	43.147290
3502.395411	376893.793818	43.152295
3501.882253	376870.177552	43.157300
3502.558603	376839.950503	43.162305
3502.372156	376831.649068	43.167309
3502.573972	376804.492772	43.172314
3502.190807	376785.072253	43.177319
3502.289580	376750.388754	43.182324
3502.493982	376727.651221	43.187329
3502.393051	376706.129490	43.192333
3502.562930	376682.686147	43.197338
3502.527878	376668.036996	43.202343
3502.240227	376634.581790	43.207348
3502.160367	376605.792853	43.212353
3502.088105	376588.838223	43.217357
3502.095175	376560.569071	43.222362
3502.207728	376546.277856	43.227367
3502.525844	376528.906867	43.232372
3502.453730	376500.319797	43.237377
3502.022984	376487.129023	43.242381
3502.059175	376459.033020	43.247386
3502.243344	376441.886005	43.252391
3502.144835	376419.881102	43.257396
3502.315323	376397.834322	43.262401
3502.091870	376373.740766	43.267405
3501.837929	376353.080708	43.272410
3501.969251	376340.488151	43.277415
3502.036319	376320.387675	43.282420
3502.042452	376313.173640	43.287425
3501.979054	376294.185576	43.292429
3502.218655	376266.438695	43.297434
3502.035731	376254.580757	43.302439
3501.869560	376236.243605	43.307444
3502.090634	376224.627567	43.312449
3501.817904	376192.718795	43.317453
3501.882534	376180.111144	43.322458
3501.778210	376156.659217	43.327463
3502.070957	376146.428911	43.332468
3502.150369	376117.335284	43.337473
3501.662840	376116.573052	43.342477
3502.084731	376088.696028	43.347482
3502.220510	376072.419860	43.352487
3501.983851	376053.814169	43.357492
3502.132139	376033.446854	43.362497
3502.116131	376013.841652	43.367501
3501.940504	375991.746805	43.372506
3502.133308	375975.639496	43.377511
3501.924632	375960.356613	43.382516
3501.865529	375941.494626	43.387521
3501.442591	375927.515002	43.392525
3502.027578	375905.631908	43.397530
3502.086645	375901.533572	43.402535
3501.731677	375876.291695	43.407540
3501.870511	375866.110633	43.412545
3501.756180	375844.361711	43.417549
3501.974465	375820.884690	43.422554
3502.190980	375810.539125	43.427559
3502.039701	375787.703757	43.432564
3501.932561	375770.754041	43.437569
3501.811000	375757.362403	43.442573
3502.245749	375742.131665	43.447578
3501.928215	375717.874372	43.452583
3501.890412	375701.751987	43.457588
3501.746465	375672.972029	43.462593
3501.642269	375678.906256	43.467597
3502.135956	375656.529190	43.472602
3502.297471	375637.607261	43.477607
3502.133577	375623.434775	43.482612
3502.056839	375587.532544	43.487617
3502.012944	375581.850042	43.492621
3501.998998	375556.377006	43.497626
3502.045550	375544.178257	43.502631
3501.991257	375522.673725	43.507636
3501.845820	375498.618047	43.512641
3501.854734	375483.224838	43.517645
3501.722918	375459.827384	43.522650
3501.838116	375456.812409	43.527655
3501.908567	375430.818139	43.532660
3502.111402	375415.572509	43.537665
3502.175140	375396.030648	43.542669
3501.954533	375371.478570	43.547674
3502.158904	375350.543232	43.552679
3502.367297	375336.388862	43.557684
3501.950420	375316.388348	43.562689
3502.222553	375304.662374	43.567693
3502.033507	375270.174162	43.572698
3502.466511	375260.175690	43.577703
3501.967057	375232.695155	43.582708
3502.343462	375214.704669	43.587713
3501.803877	375190.760852	43.592717
3501.854036	375168.731797	43.597722
3502.402766	375145.253570	43.602727
3502.014509	375141.250128	43.607732
3502.259144	375114.771260	43.612737
3502.096482	375108.599151	43.617741
3502.003570	375077.143673	43.622746
3502.042634	375070.330575	43.627751
3502.008416	375053.140467	43.632756
3502.114068	375027.368929	43.637761
3502.332263	375011.917486	43.642765
3501.982154	374991.779345	43.647770
3502.043683	374966.192413	43.652775
3501.542849	374958.040923	43.657780
3501.741822	374947.900958	43.662785
3502.384650	374930.656216	43.667789
3502.071727	374902.409729	43.672794
3501.986902	374886.167180	43.677799
3501.986878	374865.110877	43.682804
3501.982240	374839.330925	43.687809
3501.807960	374827.623414	43.692813
3501.963104	374809.235297	43.697818
3502.081393	374798.295039	43.702823
3501.973040	374774.182150	43.707828
3502.154601	374750.913120	43.712833
3501.849008	374737.651215	43.717837
3501.930718	374717.039277	43.722842
3501.876674	374709.859580	43.727847
3501.683996	374682.635548	43.732852
3501.681338	374665.973683	43.737857
3501.783685	374662.503423	43.742861
3501.512769	374633.945322	43.747866
3502.114905	374623.971100	43.752871
3501.788059	374612.236438	43.757876
3502.052845	374592.535715	43.762881
3501.430400	374584.352236	43.767885
3501.926740	374556.665260	43.772890
3501.565553	374552.581317	43.777895
3501.937697	374547.468858	43.782900
3502.043327	374519.995044	43.787905
3502.129550	374501.693645	43.792909
3502.163793	374487.083332	43.797914
3501.915919	374466.497092	43.802919
3502.152235	374451.423515	43.807924
3502.089587	374428.319212	43.812929
3502.468446	374408.905407	43.817933
3502.387246	374381.054124	43.822938
3502.281962	374357.778596	43.827943
3502.205311	374340.010437	43.832948
3502.115938	374308.451921	43.837953
3502.288026	374296.283880	43.842957
3502.055905	374285.169343	43.847962
3502.076728	374255.549438	43.852967
3501.746387	374242.087941	43.857972
3502.644835	374221.907342	43.862977
3502.319378	374205.651032	43.867981
3502.145811	374174.207064	43.872986
3502.171657	374157.210249	43.877991
3502.047858	374136.960058	43.882996
3502.128697	374116.347803	43.888001
3502.171335	374095.411271	43.893005
3501.982763	374068.693998	43.898010
3502.291451	374048.376441	43.903015
3501.945957	374027.728860	43.908020
3502.031604	374007.090374	43.913025
3502.095188	373995.701099	43.918029
3501.997781	373973.236835	43.923034
3501.939954	373960.545610	43.928039
3501.933258	373941.496279	43.933044
3501.830841	373908.999511	43.938049
3501.835326	373908.567057	43.943053
3501.910434	373885.466260	43.948058
3501.754850	373879.089566	43.953063
3501.932970	373860.087620	43.958068
3501.852591	373842.802332	43.963073
3501.403889	373835.887024	43.968077
3501.762921	373810.786131	43.973082
3501.929565	373799.914152	43.978087
3502.002021	373788.218602	43.983092
3502.148895	373767.189398	43.988097
3501.837119	373758.449311	43.993101
3502.013321	373735.434259	43.998106
3501.991909	373714.431202	44.003111
3501.621350	373691.602800	44.008116
3501.728660	373669.487442	44.013121
3501.372167	373678.687268	44.018125
3501.477134	373646.437327	44.023130
3501.897445	373642.638049	44.028135
3501.609563	373634.935640	44.033140
3501.503653	373609.424297	44.038145
3501.736374	373596.306678	44.043149
3501.538937	373587.320135	44.048154
3501.974048	373575.720467	44.053159
3502.162381	373555.472077	44.058164
3502.327668	373534.236622	44.063169
3502.152411	373519.251979	44.068173
3502.199862	373493.919872	44.073178
3501.783191	373476.127863	44.078183
3502.103056	373465.714528	44.083188
3502.118623	373433.529052	44.088193
3502.115600	373423.699369	44.093197
3501.867609	373405.093632	44.098202
3502.130590	373394.231903	44.103207
3501.951872	373371.347980	44.108212
3502.208129	373348.650363	44.113217
3502.204258	373324.824753	44.118221
3502.322425	373309.768935	44.123226
3502.558187	373288.827138	44.128231
3502.123345	373262.909438	44.133236
3502.212061	373235.259162	44.138241
3502.149075	373213.703365	44.143245
3501.716941	373206.785320	44.148250
3502.125983	373184.546416	44.153255
3501.882969	373163.831435	44.158260
3502.124279	373152.718971	44.163265
3502.011393	373127.208266	44.168269
3502.187312	373111.736932	44.173274
3502.162409	373084.637614	44.178279
3502.111562	373062.343170	44.183284
3502.055636	373047.593715	44.188289
3502.158911	373034.419768	44.193293
3502.208877	373006.673688	44.198298
3501.778374	372986.902201	44.203303
3501.609853	372967.166137	44.208308
3501.997200	372961.288976	44.213313
3501.576249	372949.441237	44.218317
3501.903967	372929.424713	44.223322
3502.224798	372914.464151	44.228327
3502.192064	372890.820468	44.233332
3502.111622	372865.812504	44.238337
3501.864049	372851.600799	44.243341
3501.954813	372839.038344	44.248346
3502.024635	372807.326325	44.253351
3501.856485	372795.566189	44.258356
3502.156352	372772.835911	44.263361
3501.834825	372760.058159	44.268365
3501.634650	372749.573070	44.273370
3501.867140	372722.966779	44.278375
3502.092593	372715.666862	44.283380
3501.963417	372688.735792	44.288385
3502.077515	372678.328780	44.293389
3502.038274	372661.595187	44.298394
3502.073243	372640.303119	44.303399
3502.159600	372626.090137	44.308404
3502.017489	372597.128848	44.313409
3502.375528	372592.323046	44.318413
3502.173314	372576.326013	44.323418
3502.385856	372547.766717	44.328423
3502.099169	372527.210465	44.333428
3501.834858	372495.905710	44.338433
3501.967240	372496.012173	44.343437
3501.981465	372469.998446	44.348442
3501.998902	372448.023105	44.353447
3501.817843	372434.181864	44.358452
3501.805362	372411.880925	44.363457
3501.525772	372408.520620	44.368461
3501.841672	372386.854414	44.373466
3501.846376	372367.675212	44.378471
3501.553090	372358.576174	44.383476
3501.668020	372331.682977	44.388481
3501.750609	372323.262096	44.393485
3501.653992	372318.399987	44.398490
3501.661269	372303.665702	44.403495
3501.574842	372289.758859	44.408500
3501.765646	372276.774148	44.413505
3501.927668	372259.450147	44.418509
3501.620456	372250.302436	44.423514
3501.943107	372232.572390	44.428519
3501.854001	372210.943669	44.433524
3502.151388	372187.070199	44.438529
3501.763050	372178.874969	44.443533
3501.879128	372150.558895	44.448538
3502.166172	372138.651439	44.453543
3501.973236	372124.151433	44.458548
3501.897163	372100.869452	44.463553
3502.064965	372074.602836	44.468557
3502.172413	372067.905365	44.473562
3501.864970	372042.652557	44.478567
3501.857741	372035.134647	44.483572
3501.718791	372007.696389	44.488577
3501.682627	371996.143996	44.493581
3501.618787	371978.042091	44.498586
3501.810667	371956.801287	44.503591
3501.758854	371952.135361	44.508596
3501.910890	371940.833086	44.513601
3501.769086	371925.207312	44.518605
3501.772553	371912.861242	44.523610
3502.071230	371893.381942	44.528615
3501.793270	371885.017035	44.533620
3502.016288	371856.429995	44.538625
3501.795124	371843.458384	44.543629
3501.884940	371828.431577	44.548634
3502.142019	371795.368330	44.553639
3501.409465	371805.135346	44.558644
3501.633189	371782.111276	44.563649
3501.590504	371758.315761	44.568653
3501.602037	371756.866073	44.573658
3501.885101	371752.046392	44.578663
3501.712632	371729.744399	44.583668
3501.788855	371725.337940	44.588673
3501.780612	371704.153488	44.593677
3501.497727	371687.330209	44.598682
3502.058634	371666.514409	44.603687
3501.670180	371655.067501	44.608692
3501.844308	371632.711495	44.613697
3501.928265	371623.299484	44.618701
3501.751896	371611.413111	44.623706
3501.743703	371592.743436	44.628711
3501.526628	371584.673796	44.633716
3501.689045	371558.712364	44.638721
3501.830275	371548.097485	44.643725
3501.947591	371529.509848	44.648730
3502.143637	371510.401891	44.653735
3501.881043	371497.461969	44.658740
3501.904765	371478.609431	44.663745
3501.674254	371473.869621	44.668749
3501.525984	371449.378993	44.673754
3501.626307	371427.288337	44.678759
3501.371914	371426.718308	44.683764
3501.419096	371420.233283	44.688769
3501.515542	371394.561396	44.693773
3501.525878	371392.019550	44.698778
3501.706833	371373.447309	44.703783
3501.914842	371370.519059	44.708788
3501.624347	371349.733901	44.713793
3501.680070	371346.219676	44.718797
3501.832155	371323.485808	44.723802
3501.965835	371307.918432	44.728807
3501.596128	371291.235439	44.733812
3501.998739	371275.753210	44.738817
3501.922088	371271.065632	44.743821
3501.848285	371244.988249	44.748826
3502.121005	371232.955622	44.753831
3501.968806	371212.834724	44.758836
3501.891799	371189.679142	44.763841
3501.746484	371185.434087	44.768845
3501.490948	371165.354639	44.773850
3502.041569	371149.417456	44.778855
3501.700903	371132.196382	44.783860
3501.782136	371113.410858	44.788865
3501.535171	371118.911024	44.793869
3501.557615	371098.254804	44.798874
3501.894479	371076.508110	44.803879
3501.767573	371073.809769	44.808884
3501.977855	371044.537994	44.813889
3501.971099	371036.943531	44.818893
3501.569253	371024.380704	44.823898
3501.803364	371001.506795	44.828903
3501.399419	370989.655570	44.833908
3501.809588	370975.619987	44.838913
3502.191243	370959.327940	44.843917
3501.525337	370951.759816	44.848922
3502.098876	370920.500732	44.853927
3501.580088	370908.159277	44.858932
3501.998025	370890.794603	44.863937
3501.954473	370870.478729	44.868941
3502.000591	370853.044874	44.873946
3501.801298	370839.053256	44.878951
3501.708907	370824.867172	44.883956
3501.633613	370811.364314	44.888961
3501.573514	370795.369545	44.893965
3501.717973	370787.014783	44.898970
3501.721434	370784.270724	44.903975
3501.634285	370763.961556	44.908980
3501.449371	370750.856779	44.913985
3501.512524	370740.329954	44.918989
3501.425273	370722.840562	44.923994
3501.899110	370709.633256	44.928999
3501.603954	370703.404565	44.934004
3501.793922	370679.013050	44.939009
3501.838621	370665.288220	44.944013
3501.641337	370661.228997	44.949018
3501.925357	370633.571148	44.954023
3501.761465	370627.245803	44.959028
3501.976492	370619.870751	44.964033
3501.637602	370595.612268	44.969037
3501.770291	370579.409550	44.974042
3501.884996	370561.685401	44.979047
3501.790590	370549.785822	44.984052
3501.994782	370537.052257	44.989057
3501.963954	370517.445450	44.994061
3501.971948	370496.918055	44.999066
3502.026607	370477.221705	45.004071
3501.579916	370463.674858	45.009076
3501.792151	370448.806086	45.014081
3501.438458	370431.484993	45.019085
3501.586515	370424.653791	45.024090
3502.004451	370409.905412	45.029095
3502.315574	370403.023426	45.034100
3501.999778	370376.169970	45.039105
3502.116316	370353.034386	45.044109
3502.029133	370331.048256	45.049114
3501.858598	370316.213574	45.054119
3501.667533	370309.308096	45.059124
3501.793631	370279.261103	45.064129
3502.000377	370275.367588	45.069133
3501.586345	370250.561612	45.074138
3501.775161	370224.112161	45.079143
3501.797098	370228.884749	45.084148
3501.675435	370206.980099	45.089153
3501.870074	370194.171654	45.094157
3501.808778	370177.084347	45.099162
3502.138526	370158.234108	45.104167
3501.907848	370145.110765	45.109172
3501.980430	370121.829408	45.114177
3501.745792	370100.933014	45.119181
3502.017191	370088.925508	45.124186
3502.073222	370066.485015	45.129191
3501.788765	370066.757971	45.134196
3501.851333	370038.219450	45.139201
3501.431767	370022.737453	45.144205
3501.702816	370021.018654	45.149210
3501.521112	370003.238662	45.154215
3501.773319	369994.739878	45.159220
3502.130161	369978.374913	45.164225
3502.176668	369961.905805	45.169229
3501.710848	369937.793526	45.174234
3501.823258	369920.297969	45.179239
3501.705869	369909.900546	45.184244
3501.542440	369900.907518	45.189249
3501.756498	369867.569248	45.194253
3501.630181	369861.949204	45.199258
3501.705210	369857.313999	45.204263
3501.689807	369848.704388	45.209268
3501.827636	369826.581232	45.214273
3502.105064	369826.055432	45.219277
3502.071259	369792.349175	45.224282
3501.931471	369774.435494	45.229287
3501.568944	369762.577304	45.234292
3501.588989	369744.105240	45.239297
3501.752851	369733.562368	45.244301
3501.706632	369713.347691	45.249306
3501.662902	369696.003314	45.254311
3501.627594	369683.611488	45.259316
3501.967625	369659.017907	45.264321
3501.787506	369651.145194	45.269325
3501.284014	369637.860831	45.274330
3501.653080	369614.482110	45.279335
3501.712201	369616.378303	45.284340
3501.821222	369595.199416	45.289345
3501.757902	369578.670961	45.294349
3501.939249	369569.776604	45.299354
3501.980698	369552.088625	45.304359
3501.557296	369525.098674	45.309364
3502.027932	369515.676595	45.314369
3501.938542	369504.207671	45.319373
3501.576053	369494.889825	45.324378
3501.739972	369474.642277	45.329383
3501.676396	369452.524765	45.334388
3501.333339	369449.682070	45.339393
3501.354754	369452.879780	45.344397
3501.061177	369433.033654	45.349402
3501.512634	369402.681052	45.354407
3501.138939	369407.058059	45.359412
3501.517543	369391.629342	45.364417
3501.562760	369392.562335	45.369421
3501.484136	369374.384835	45.374426
3501.997376	369355.607128	45.379431
3501.438649	369354.271460	45.384436
3501.739996	369327.702040	45.389441
3501.708437	369324.378978	45.394445
3501.310532	369323.119902	45.399450
3501.502433	369303.579211	45.404455
3501.390779	369293.917408	45.409460
3501.141657	369279.323053	45.414465
3501.583678	369273.944713	45.419469
3501.725664	369266.174198	45.424474
3501.688625	369253.757047	45.429479
3501.535745	369243.720569	45.434484
3501.978012	369222.159284	45.439489
3501.575515	369212.644331	45.444493
3501.673869	369197.106690	45.449498
3501.607613	369177.733110	45.454503
3501.081740	369160.387218	45.459508
3502.081483	369158.173900	45.464513
3501.798338	369142.746405	45.469517
3501.431606	369125.350323	45.474522
3501.960386	369114.725030	45.479527
3501.552488	369093.346752	45.484532
3501.536336	369067.055141	45.489537
3501.675734	369070.564799	45.494541
3501.554684	369058.770357	45.499546
3501.776532	369037.751331	45.504551
3501.770683	369026.599480	45.509556
3502.016161	369013.249084	45.514561
3501.999865	368986.373103	45.519565
3501.594105	368980.770963	45.524570
3501.655644	368956.906049	45.529575
3501.661761	368948.851728	45.534580
3501.527169	368944.960337	45.539585
3501.877192	368921.304552	45.544589
3501.999905	368905.000807	45.549594
3501.892416	368894.855522	45.554599
3501.888067	368878.088835	45.559604
3501.725237	368862.667871	45.564609
3501.697177	368842.754609	45.569613
3501.678903	368825.939248	45.574618
3501.669665	368813.720821	45.579623
3501.493815	368797.311042	45.584628
3501.580998	368781.444645	45.589633
3501.646684	368783.289062	45.594637
3501.558993	368767.551490	45.599642
3502.074918	368739.042733	45.604647
3501.745766	368734.546456	45.609652
3501.822241	368715.683861	45.614657
3501.843894	368695.737355	45.619661
3501.896253	368691.105487	45.624666
3501.769351	368670.089650	45.629671
3501.597686	368660.132104	45.634676
3501.819760	368651.739230	45.639681
3501.795494	368625.981986	45.644685
3501.840567	368623.713944	45.649690
3501.515391	368592.084033	45.654695
3501.169682	368584.084358	45.659700
3501.462045	368571.996732	45.664705
3501.789484	368575.197730	45.669709
3501.639201	368558.224916	45.674714
3501.579495	368546.674769	45.679719
3501.577722	368543.067520	45.684724
3501.448704	368521.924875	45.689729
3501.525151	368513.580027	45.694733
3501.192685	368513.098301	45.699738
3501.204508	368499.733213	45.704743
3501.364432	368497.066206	45.709748
3501.132936	368475.990285	45.714753
3501.450419	368464.228976	45.719757
3501.482204	368452.791582	45.724762
3501.625478	368443.318469	45.729767
3501.699721	368429.791202	45.734772
3501.712150	368416.959498	45.739777
3501.368699	368414.904333	45.744781
3501.431223	368398.660475	45.749786
3501.679597	368379.516852	45.754791
3501.246091	368379.711393	45.759796
3501.347969	368366.713314	45.764801
3501.540046	368354.666607	45.769805
3501.291465	368345.965798	45.774810
3501.644503	368314.534908	45.779815
3501.502888	368261.916366	45.784820
3501.346570	368163.722007	45.789825
3500.982235	368022.090137	45.794829
3500.368795	367827.651647	45.799834
3500.618125	367592.986419	45.804839
3499.885543	367313.375433	45.809844
3498.908635	366992.335779	45.814849
3497.774415	366626.727453	45.819853
3496.896525	366236.708801	45.824858
3496.339465	365798.766508	45.829863
3495.204223	365328.003827	45.834868
3494.353793	364811.605923	45.839873
3493.208985	364254.513707	45.844877
3491.687122	363679.987694	45.849882
3490.655083	363054.325041	45.854887
3489.043005	362409.198508	45.859892
3487.358075	361716.270468	45.864897
3485.806213	360993.497362	45.869901
3483.915759	360258.358200	45.874906
3482.286033	359480.415434	45.879911
3480.344837	358677.722623	45.884916
3478.274068	357843.057283	45.889921
3476.593993	356971.532483	45.894925
3474.082016	356085.752543	45.899930
3472.378469	355177.581933	45.904935
3470.055899	354240.886632	45.909940
3467.748277	353283.953706	45.914945
3465.236430	352285.743179	45.919949
3462.791911	351282.839343	45.924954
3460.534540	350259.615036	45.929959
3458.364256	349219.185610	45.934964
3455.481444	348152.572937	45.939969
3453.075837	347068.665722	45.944973
3450.267317	345962.616455	45.949978
3447.524974	344832.392577	45.954983
3444.722106	343699.547337	45.959988
3441.980063	342553.230245	45.964993
3439.036061	341385.598743	45.969997
3436.349927	340210.463360	45.975002
3433.196626	339007.567881	45.980007
3430.313974	337810.820387	45.985012
3427.307868	336586.562039	45.990017
3424.492589	335356.383945	45.995021
3421.244219	334110.540701	46.000026
3418.001475	332855.321276	46.005031
3414.756745	331597.237556	46.010036
3411.439629	330327.194980	46.015041
3408.376908	329038.248920	46.020045
3405.504295	327756.989355	46.025050
3402.270488	326457.531695	46.030055
3398.845141	325151.778870	46.035060
3395.535628	323840.191775	46.040065
3392.175007	322517.682972	46.045069
3388.628786	321197.069593	46.050074
3385.410353	319857.105188	46.055079
3381.644375	318528.455475	46.060084
3378.420619	317185.484017	46.065089
3375.214419	315836.286555	46.070093
3371.275566	314489.681913	46.075098
3368.064187	313130.227418	46.080103
3364.799582	311778.909794	46.085108
3361.053926	310416.686427	46.090113
3357.608231	309054.097950	46.095117
3354.011492	307690.578939	46.100122
3350.651230	306316.857152	46.105127
3347.218331	304948.301119	46.110132
3343.610852	303569.275872	46.115137
3339.912189	302188.981462	46.120141
3336.051846	300808.167500	46.125146
3332.456140	299420.914253	46.130151
3328.653715	298049.184647	46.135156
3325.207327	296678.079007	46.140161
3321.851351	295281.345359	46.145165
3317.585927	293912.847352	46.150170
3314.600664	292522.329231	46.155175
3310.765315	291146.752486	46.160180
3306.992178	289756.676571	46.165185
3303.491582	288371.262933	46.170189
3299.545305	286989.020479	46.175194
3296.215994	285609.733774	46.180199
3292.064685	284219.014437	46.185204
3288.300709	282841.980415	46.190209
3285.109310	281458.185883	46.195213
3281.131066	280081.565530	46.200218
3277.551605	278694.801080	46.205223
3273.861043	277310.956987	46.210228
3269.963954	275935.421226	46.215233
3266.676326	274558.494298	46.220237
3262.398689	273177.268385	46.225242
3258.966419	271799.988231	46.230247
3255.182869	270444.512106	46.235252
3251.424029	269074.625317	46.240257
3247.435346	267697.038930	46.245261
3243.603513	266331.580422	46.250266
3240.001496	264961.153030	46.255271
3236.342958	263598.584980	46.260276
3232.595011	262235.657142	46.265281
3228.800702	260870.733649	46.270285
3224.686654	259519.518890	46.275290
3221.255102	258164.210174	46.280295
3217.372065	256823.192684	46.285300
3213.870052	255467.229898	46.290305
3210.161404	254118.161876	46.295309
3206.010293	252773.250234	46.300314
3202.702525	251425.368559	46.305319
3198.714849	250093.447363	46.310324
3195.466498	248761.960837	46.315329
3192.154969	247415.957629	46.320333
3187.482974	246088.391465	46.325338
3183.776456	244742.380304	46.330343
3180.199647	243415.645365	46.335348
3176.110684	242087.225213	46.340353
3172.560093	240757.135193	46.345357
3168.916616	239435.432270	46.350362
3164.810820	238116.877146	46.355367
3161.368277	236798.340897	46.360372
3157.431656	235487.313722	46.365377
3153.802391	234179.647453	46.370381
3149.877560	232876.735405	46.375386
3146.137204	231560.114861	46.380391
3142.168784	230264.692092	46.385396
3138.752413	228966.150751	46.390401
3134.864658	227664.650624	46.395405
3131.074585	226382.898505	46.400410
3127.552698	225089.643320	46.405415
3123.471880	223794.565209	46.410420
3119.725187	222518.817847	46.415425
3116.245447	221232.256844	46.420429
3111.917520	219951.687528	46.425434
3108.188558	218676.681433	46.430439
3103.995336	217409.009025	46.435444
3100.506102	216159.516935	46.440449
3097.228785	214890.894008	46.445453
3093.382941	213637.186563	46.450458
3089.410580	212376.576034	46.455463
3085.561416	211125.527657	46.460468
3081.894420	209878.302247	46.465473
3078.338718	208640.921739	46.470477
3074.449398	207398.505957	46.475482
3071.041774	206157.575691	46.480487
3066.992103	204930.021405	46.485492
3063.137436	203696.255838	46.490497
3059.551626	202462.507586	46.495501
3055.580185	201237.359533	46.500506
3052.165455	200012.312124	46.505511
3048.029972	198791.180884	46.510516
3044.437156	197589.507919	46.515521
3040.516870	196376.716126	46.520525
3036.384787	195174.587257	46.525530
3032.889007	193965.468922	46.530535
3029.342484	192774.501423	46.535540
3025.303121	191583.163690	46.540545
3021.348665	190388.310424	46.545549
3017.813074	189206.416905	46.550554
3014.068942	188023.473355	46.555559
3010.088290	186858.939338	46.560564
3006.417845	185688.105801	46.565569
3002.989033	184519.387065	46.570573
2998.857310	183353.185068	46.575578
2995.098490	182190.045667	46.580583
2991.171542	181030.307955	46.585588
2987.222056	179887.139113	46.590593
2983.642948	178741.584792	46.595597
2979.312164	177612.763674	46.600602
2975.562234	176464.898370	46.605607
2971.956476	175354.021585	46.610612
2967.969052	174228.515812	46.615617
2964.091938	173121.658629	46.620621
2960.209095	172011.661082	46.625626
2956.351571	170910.319380	46.630631
2952.628697	169813.695722	46.635636
2948.851499	168726.784121	46.640641
2944.764501	167638.091488	46.645645
2940.662341	166573.832459	46.650650
2937.214943	165491.107458	46.655655
2933.242018	164427.778213	46.660660
2928.983415	163367.514334	46.665665
2925.316659	162322.411271	46.670669
2921.132158	161282.089679	46.675674
2917.238274	160241.345397	46.680679
2913.315693	159207.763173	46.685684
2909.220385	158194.754582	46.690689
2905.392685	157184.712231	46.695693
2901.261676	156186.990320	46.700698
2897.300294	155190.022592	46.705703
2893.516605	154216.766710	46.710708
2889.207218	153246.994452	46.715713
2885.783758	152269.719895	46.720717
2881.304801	151319.669330	46.725722
2877.393876	150372.168334	46.730727
2873.534120	149433.736493	46.735732
2868.904885	148512.874449	46.740737
2865.270047	147592.471800	46.745741
2860.545884	146694.192447	46.750746
2856.731380	145805.890495	46.755751
2852.540020	144926.824194	46.760756
2848.816587	144066.124941	46.765761
2844.239440	143206.578574	46.770765
2839.479413	142383.732605	46.775770
2835.580473	141467.986899	46.780775
2831.200698	140658.317912	46.785780
2826.478155	139871.515639	46.790785
2822.206947	139087.531538	46.795789
2817.935555	138330.176259	46.800794
2813.870851	137592.266423	46.805799
2809.315517	136861.111163	46.810804
2804.941148	136151.337844	46.815809
2800.463354	135443.614471	46.820813
2796.202575	134768.537573	46.825818
2792.016109	134092.696004	46.830823
2788.219021	133440.885445	46.835828
2783.958601	132799.524287	46.840833
2780.033605	132162.394537	46.845837
2776.026872	131551.669566	46.850842
2772.163701	130934.532460	46.855847
2768.187736	130328.615674	46.860852
2764.180345	129750.111617	46.865857
2760.786377	129154.742323	46.870861
2756.978741	128582.621310	46.875866
2753.575662	128015.291338	46.880871
2750.083432	127431.854681	46.885876
2746.239657	126874.262951	46.890881
2742.579311	126311.231884	46.895885
2739.097734	125745.980364	46.900890
2735.922057	125197.770396	46.905895
2732.219863	124630.266648	46.910900
2728.548597	124084.412833	46.915905
2724.700863	123525.201614	46.920909
2720.974277	122983.479455	46.925914
2717.908864	122439.385314	46.930919
2714.419858	121901.202038	46.935924
2710.403197	121357.423527	46.940929
2706.761099	120814.866050	46.945933
2703.296561	120288.070566	46.950938
2700.020200	119740.155463	46.955943
2696.561012	119211.593501	46.960948
2693.099710	118681.309719	46.965953
2689.470073	118142.285162	46.970957
2685.605646	117611.112637	46.975962
2682.060583	117089.015373	46.980967
2678.830355	116561.573846	46.985972
2675.297471	116036.208693	46.990977
2671.756931	115497.640686	46.995981
2668.094640	114983.080728	47.000986
2664.505731	114455.585183	47.005991
2661.105469	113932.009556	47.010996
2657.064768	113414.275531	47.016001
2653.871800	112888.699181	47.021005
2650.072605	112377.821070	47.026010
2646.597821	111857.122449	47.031015
2643.101712	111337.540870	47.036020
2639.486507	110837.552170	47.041025
2636.111476	110307.821113	47.046029
2632.508534	109802.670668	47.051034
2628.829325	109288.322167	47.056039
2625.138541	108789.022758	47.061044
2620.883222	108295.882486	47.066049
2617.509099	107794.514034	47.071053
2613.568537	107302.267009	47.076058
2609.976077	106813.023867	47.081063
2606.201461	106325.913605	47.086068
2602.405412	105856.216531	47.091073
2598.838578	105380.363143	47.096077
2594.670748	104905.626932	47.101082
2591.395781	104431.635576	47.106087
2587.725509	103978.241356	47.111092
2583.524869	103516.241354	47.116097
2579.896737	103064.772412	47.121101
2575.609324	102631.321862	47.126106
2571.891467	102187.365584	47.131111
2568.605841	101758.905750	47.136116
2564.731034	101325.878497	47.141121
2561.599659	100891.101678	47.146125
2557.419113	100464.234363	47.151130
2554.049071	100049.371766	47.156135
2550.528093	99618.091610	47.161140
2546.943729	99205.268650	47.166145
2543.484289	98791.719836	47.171149
2540.027100	98372.927109	47.176154
2536.500449	97951.774102	47.181159
2533.166622	97535.921693	47.186164
2529.480751	97113.787881	47.191169
2525.979950	96699.446672	47.196173
2522.441651	96288.662395	47.201178
2519.066391	95875.926478	47.206183
2515.864155	95463.804487	47.211188
2512.013662	95047.595230	47.216193
2508.756945	94624.970708	47.221197
2505.078422	94214.667663	47.226202
2502.113009	93799.925884	47.231207
2498.588646	93374.729711	47.236212
2494.794048	92963.216120	47.241217
2491.415798	92534.018882	47.246221
2488.008175	92120.321687	47.251226
2484.605646	91694.825002	47.256231
2481.381947	91276.485534	47.261236
2477.709481	90851.652630	47.266241
2474.050479	90426.048568	47.271245
2470.778375	90000.809627	47.276250
2467.432261	89570.201080	47.281255
2463.850190	89151.565860	47.286260
2460.481927	88729.078990	47.291265
2457.339399	88293.171895	47.296269
2453.872664	87875.781857	47.301274
2450.327765	87431.005906	47.306279
2446.902713	86995.975093	47.311284
2443.094385	86571.046797	47.316289
2439.830680	86138.315838	47.321293
2436.374092	85703.004332	47.326298
2432.961787	85260.756238	47.331303
2429.197328	84824.083057	47.336308
2425.764681	84392.865413	47.341313
2422.612760	83960.429168	47.346317
2418.872077	83522.565296	47.351322
2415.429656	83084.826867	47.356327
2411.715408	82644.660481	47.361332
2408.329789	82197.184033	47.366337
2405.221158	81761.979969	47.371341
2401.337220	81320.882550	47.376346
2397.614323	80888.162874	47.381351
2394.125706	80443.461243	47.386356
2391.059910	80010.182942	47.391361
2387.964161	79563.224177	47.396365
2383.953111	79118.294802	47.401370
2380.559867	78667.561097	47.406375
2377.154018	78229.156267	47.411380
2373.445409	77792.647099	47.416385
2370.133917	77340.449195	47.421389
2366.495626	76891.433820	47.426394
2363.023822	76441.561757	47.431399
2359.561737	76003.150607	47.436404
2355.662208	75557.398233	47.441409
2352.811635	75107.934229	47.446413
2349.163903	74666.767179	47.451418
2345.508018	74213.011557	47.456423
2342.336493	73767.442261	47.461428
2338.629528	73322.078021	47.466433
2335.317917	72876.113700	47.471437
2331.640631	72436.232563	47.476442
2328.287239	71971.814636	47.481447
2325.070995	71521.807787	47.486452
2321.261719	71072.891316	47.491457
2317.617206	70613.075606	47.496461
2313.841054	70164.937733	47.501466
2310.965496	69720.368452	47.506471
2307.342255	69255.234522	47.511476
2303.507562	68808.043316	47.516481
2300.505266	68353.417505	47.521485
2297.321144	67903.811053	47.526490
2293.328106	67442.722073	47.531495
2290.032534	66980.580722	47.536500
2286.409748	66526.610733	47.541505
2283.115682	66056.938760	47.546509
2279.637395	65605.355703	47.551514
2276.234718	65146.939434	47.556519
2272.368393	64688.901964	47.561524
2269.068628	64223.327067	47.566529
2265.816905	63748.855159	47.571533
2262.024732	63296.721396	47.576538
2258.096036	62820.633506	47.581543
2254.907181	62363.751751	47.586548
2251.166090	61902.153863	47.591553
2248.104109	61434.753693	47.596557
2244.377300	60973.450190	47.601562
2240.804065	60520.032154	47.606567
2237.674151	60055.873487	47.611572
2233.919013	59595.774316	47.616577
2230.684599	59132.525187	47.621581
2226.884726	58666.460325	47.626586
2223.656630	58202.517280	47.631591
2220.120850	57733.878460	47.636596
2216.301470	57265.248478	47.641601
2212.915547	56796.858397	47.646605
2209.438067	56332.419186	47.651610
2206.141935	55874.806743	47.656615
2202.954223	55393.609674	47.661620
2199.438040	54938.530229	47.666625
2196.000234	54468.430244	47.671629
2192.253308	53988.382881	47.676634
2188.648593	53514.185114	47.681639
2185.477595	53044.763526	47.686644
2181.574478	52576.156763	47.691649
2178.091516	52101.340613	47.696653
2174.905408	51638.255292	47.701658
2171.012953	51163.921653	47.706663
2167.674812	50692.112224	47.711668
2164.448382	50217.377174	47.716673
2160.850448	49737.191255	47.721677
2156.933911	49266.148037	47.726682
2153.700408	48786.020454	47.731687
2149.851262	48310.806513	47.736692
2146.418075	47842.400377	47.741697
2143.360643	47365.490986	47.746701
2139.781734	46904.350890	47.751706
2136.064115	46429.428597	47.756711
2132.817848	45953.054053	47.761716
2129.277750	45474.001981	47.766721
2125.606762	44994.111698	47.771725
2122.318235	44521.680651	47.776730
2118.777191	44047.954519	47.781735
2115.366629	43564.021304	47.786740
2111.336551	43079.148765	47.791745
2108.332473	42607.075617	47.796749
2104.796781	42131.404885	47.801754
2101.328276	41653.939538	47.806759
2097.938184	41165.205048	47.811764
2094.041163	40686.343760	47.816769
2090.775315	40203.007215	47.821773
2087.144891	39742.195220	47.826778
2083.746061	39250.252476	47.831783
2080.598036	38768.799838	47.836788
2077.017241	38295.248599	47.841793
2073.252728	37812.772075	47.846797
2069.674580	37334.645311	47.851802
2066.446390	36849.995901	47.856807
2062.996400	36355.553503	47.861812
2059.561413	35875.807902	47.866817
2056.145432	35382.409739	47.871821
2052.584431	34903.973491	47.876826
2048.677946	34420.416810	47.881831
2045.536225	33927.998711	47.886836
2041.870417	33449.732181	47.891841
2038.452306	32960.821483	47.896845
2034.689555	32481.153363	47.901850
2030.929598	31995.183254	47.906855
2027.258764	31515.865278	47.911860
2023.819006	31030.989645	47.916865
2020.692795	30551.241605	47.921869
2017.159446	30069.058474	47.926874
2013.124876	29591.812572	47.931879
2010.105431	29109.584598	47.936884
2006.514962	28646.442156	47.941889
2002.732712	28154.729623	47.946893
1999.299135	27680.907230	47.951898
1996.107254	27196.641122	47.956903
1992.412869	26719.529732	47.961908
1988.575361	26245.043335	47.966913
1985.276498	25761.860949	47.971917
1981.795655	25285.466138	47.976922
1978.317523	24809.405306	47.981927
1974.948958	24329.315641	47.986932
1971.152442	23857.052281	47.991937
1967.869988	23379.746916	47.996941
1964.271710	22908.349429	48.001946
1960.369245	22426.545137	48.006951
1956.914454	21947.432179	48.011956
1953.075476	21485.145737	48.016961
1949.926657	21004.170987	48.021965
1946.225757	20541.511455	48.026970
1942.929596	20065.700733	48.031975
1939.468682	19589.547162	48.036980
1935.657914	19118.273385	48.041985
1932.307816	18656.876917	48.046989
1928.477910	18185.255003	48.051994
1924.929045	17718.629546	48.056999
1921.296831	17256.246261	48.062004
1917.530049	16801.529562	48.067009
1914.048428	16330.560472	48.072013
1910.377577	15877.994361	48.077018
1906.959301	15421.565183	48.082023
1903.185764	14961.918764	48.087028
1899.368925	14519.849796	48.092033
1895.851882	14067.232935	48.097037
1892.164727	13629.403877	48.102042
1888.289262	13193.061072	48.107047
1884.815247	12746.034782	48.112052
1880.983694	12319.880453	48.117057
1876.452229	11908.533755	48.122061
1871.515774	11521.432230	48.127066
1866.005916	11166.910372	48.132071
1860.993367	10821.862009	48.137076
1856.007011	10493.852707	48.142081
1851.283932	10174.696795	48.147085
1846.859313	9884.767228	48.152090
1842.694131	9600.917273	48.157095
1839.097935	9329.049266	48.162100
1835.104939	9073.750703	48.167105
1831.500197	8817.094323	48.172109
1827.718848	8573.196187	48.177114
1823.985296	8342.767843	48.182119
1820.739933	8102.084256	48.187124
1817.171014	7883.229803	48.192129
1814.239419	7644.943613	48.197133
1810.344902	7418.441692	48.202138
1807.186305	7185.333556	48.207143
1803.671118	6963.664881	48.212148
1800.368239	6744.485078	48.217153
1796.852480	6514.267284	48.222157
1793.912090	6295.916253	48.227162
1790.301690	6078.900032	48.232167
1787.083397	5849.163332	48.237172
1783.120510	5634.305465	48.242177
1779.775247	5402.932691	48.247181
1776.576003	5176.495891	48.252186
1773.432312	4959.186183	48.257191
1769.801463	4727.654419	48.262196
1766.321528	4516.338984	48.267201
1763.486525	4291.220419	48.272205
1759.960031	4058.747442	48.277210
1756.083463	3841.293054	48.282215
1752.946358	3616.660250	48.287220
1748.935700	3395.903223	48.292225
1745.451215	3172.829881	48.297229
1741.882980	2944.567210	48.302234
1738.594525	2732.771368	48.307239
1735.066547	2504.169452	48.312244
1731.279737	2284.881521	48.317249
1727.559523	2072.518352	48.322253
1724.314292	1864.181177	48.327258
1720.481308	1647.373005	48.332263
1716.969438	1438.620342	48.337268
1713.214674	1238.880767	48.342273
1709.740772	1029.184135	48.347277
1706.107026	828.288164	48.352282
1702.346522	633.966420	48.357287
1698.836461	434.343311	48.362292
1695.101695	257.071226	48.367297
1690.684072	85.516440	48.372301
1683.799101	-7.591994	48.377306
1671.650642	42.330044	48.382311
1665.148844	47.900939	48.387316
1661.034818	55.593192	48.392321
1658.243519	54.914068	48.397325
1656.508637	48.492922	48.402330
1653.859696	58.605161	48.407335
1651.886146	60.177863	48.412340
1648.609711	48.450686	48.417345
1645.612688	52.770587	48.422349
1642.544510	56.987672	48.427354
1638.758688	47.399347	48.432359
1635.071387	49.906322	48.437364
1631.273199	56.258630	48.442369
1628.535941	58.412098	48.447373
1625.211406	54.250484	48.452378
1621.820946	58.985957	48.457383
1619.089011	54.200609	48.462388
1615.270283	56.455963	48.467393
1611.755399	54.332925	48.472397
1608.632806	55.268236	48.477402
1605.011366	56.224242	48.482407
1601.860047	56.964711	48.487412
1597.928900	64.944876	48.492417
1594.517456	66.785672	48.497421
1591.178990	58.776008	48.502426
1587.549617	61.103132	48.507431
1584.141935	64.398643	48.512436
1580.435202	58.081932	48.517441
1577.574832	59.163090	48.522445
1574.244030	57.527087	48.527450
1570.351031	60.632385	48.532455
1566.808602	50.819531	48.537460
1563.612875	56.078344	48.542465
1560.090055	48.720632	48.547469
1557.156881	61.733928	48.552474
1553.297809	59.787851	48.557479
1549.909908	57.031298	48.562484
1545.988305	56.977355	48.567489
1542.488433	52.238776	48.572493
1539.284777	55.122890	48.577498
1535.878598	51.404258	48.582503
1532.716452	46.571989	48.587508
1529.260167	45.746446	48.592513
1525.684474	46.916798	48.597517
1522.250269	44.031419	48.602522
1518.595390	52.338734	48.607527
1515.102685	48.443751	48.612532
1511.055835	54.233666	48.617537
1507.824237	43.211371	48.622541
1504.735655	53.512254	48.627546
1501.060890	65.536847	48.632551
1498.307449	56.926788	48.637556
1493.855732	65.753596	48.642561
1490.371265	63.056371	48.647565
1487.239083	63.566085	48.652570
1483.740218	65.727374	48.657575
1480.367495	58.650023	48.662580
1476.726866	62.389915	48.667585
1473.800203	55.705038	48.672589
1469.742735	63.654250	48.677594
1466.462676	61.551624	48.682599
1462.964710	53.997072	48.687604
1459.653279	54.455595	48.692609
1455.976150	59.450828	48.697613
1452.336330	66.756080	48.702618
1448.557361	65.164536	48.707623
1445.526557	59.198211	48.712628
1442.289024	65.573996	48.717633
1438.686415	61.066551	48.722637
1435.138060	63.789194	48.727642
1431.368874	64.407552	48.732647
1427.890642	58.276758	48.737652
1424.227350	62.194184	48.742657
1421.294173	57.535091	48.747661
1417.819024	54.640278	48.752666
1413.987510	64.091877	48.757671
1410.638209	62.082291	48.762676
1407.370756	69.019545	48.767681
1403.316537	64.484323	48.772685
1399.986589	58.194414	48.777690
1396.405980	64.234465	48.782695
1393.190659	56.642257	48.787700
1389.668525	58.538262	48.792705
1386.223895	54.771850	48.797709
1382.569725	61.351688	48.802714
1378.756875	65.852370	48.807719
1375.644426	59.218569	48.812724
1371.877750	69.093506	48.817729
1368.576215	65.225729	48.822733
1365.209675	59.517312	48.827738
1361.234543	64.944907	48.832743
1358.203843	59.215855	48.837748
1354.624571	67.501922	48.842753
1351.313478	61.319814	48.847757
1347.969081	58.034505	48.852762
1344.501208	57.324678	48.857767
1340.921556	58.660175	48.862772
1337.119249	57.432939	48.867777
1333.377058	57.708591	48.872781
1330.311673	61.387429	48.877786
1326.331774	68.229939	48.882791
1323.288401	56.555126	48.887796
1319.860088	59.053453	48.892801
1316.133790	54.479861	48.897805
1312.553383	47.545597	48.902810
1309.429029	56.839669	48.907815
1305.824976	50.443749	48.912820
1302.505605	54.652493	48.917825
1298.684649	55.522527	48.922829
1295.088138	53.823512	48.927834
1291.241211	56.478746	48.932839
1288.375841	51.094124	48.937844
1284.682924	59.802831	48.942849
1281.271960	56.065994	48.947853
1277.216893	53.524050	48.952858
1274.088548	55.937725	48.957863
1270.909861	55.682756	48.962868
1266.987449	61.089496	48.967873
1263.756540	57.745405	48.972877
1260.623308	54.401930	48.977882
1256.876376	61.812444	48.982887
1253.491914	59.454017	48.987892
1249.747536	61.590267	48.992897
1246.223607	49.212007	48.997901
1242.553705	53.076691	49.002906
1238.766916	64.156960	49.007911
1236.027457	51.504738	49.012916
1232.506037	59.582489	49.017921
1228.497205	65.214651	49.022925
1225.673554	60.051327	49.027930
1221.633267	56.035975	49.032935
1218.338488	52.603759	49.037940
1214.437435	61.284757	49.042945
1210.769731	58.461069	49.047949
1207.904962	65.360959	49.052954
1204.385733	62.713473	49.057959
1200.878100	51.215354	49.062964
1197.231255	55.424459	49.067969
1193.866044	64.822465	49.072973
1190.515183	57.267206	49.077978
1186.441116	53.282428	49.082983
1183.095200	58.055285	49.087988
1179.656793	66.537726	49.092993
1176.203935	60.092980	49.097997
1172.782674	57.351157	49.103002
1168.919317	56.592180	49.108007
1165.895538	51.833332	49.113012
1162.062447	55.859463	49.118017
1158.793995	53.849978	49.123021
1155.767962	51.748977	49.128026
1151.996923	50.523226	49.133031
1148.223256	52.970921	49.138036
1144.573624	53.029711	49.143041
1141.153226	45.760529	49.148045
1137.597578	54.099868	49.153050
1134.028120	59.603534	49.158055
1130.811166	51.132121	49.163060
1127.140857	53.978173	49.168065
1123.459788	47.467725	49.173069
1119.834683	56.225991	49.178074
1116.696816	50.690824	49.183079
1113.938593	48.310866	49.188084
1110.176720	47.548755	49.193089
1106.358965	50.158337	49.198093
1103.040209	47.634682	49.203098
1098.987552	53.039560	49.208103
1095.639087	44.715175	49.213108
1092.154457	57.330250	49.218113
1088.741648	48.727985	49.223117
1085.387324	45.573969	49.228122
1081.514218	54.323385	49.233127
1078.224000	45.926662	49.238132
1074.299698	51.412800	49.243137
1071.399556	51.984506	49.248141
1067.917279	51.691395	49.253146
1064.109758	56.539275	49.258151
1060.903976	46.050873	49.263156
1057.181777	48.879697	49.268161
1053.501203	57.725694	49.273165
1050.058985	43.813030	49.278170
1046.618774	57.863830	49.283175
1043.004574	51.890303	49.288180
1039.408552	64.370866	49.293185
1035.927146	52.251780	49.298189
1032.757887	41.090164	49.303194
1029.028285	44.271312	49.308199
1025.939041	46.365714	49.313204
1022.477037	47.575364	49.318209
1018.434868	48.172987	49.323213
1014.799277	51.560960	49.328218
1011.851868	58.850196	49.333223
1008.590527	47.509930	49.338228
1004.421064	51.003153	49.343233
1001.171538	53.726771	49.348237
997.578125	55.602270	49.353242
994.072832	54.407938	49.358247
990.639420	55.492921	49.363252
987.322428	62.314517	49.368257
983.504010	61.029725	49.373261
980.294394	53.480991	49.378266
976.445008	63.182154	49.383271
973.233156	56.029228	49.388276
969.389477	62.765135	49.393281
966.505292	46.946508	49.398285
962.789177	54.029543	49.403290
959.098647	56.132130	49.408295
955.336014	57.543605	49.413300
951.800940	51.118025	49.418305
948.510347	49.466345	49.423309
945.631226	49.946208	49.428314
941.750447	51.043888	49.433319
938.103933	50.235369	49.438324
934.738908	52.021540	49.443329
931.065133	62.100319	49.448333
927.724504	51.477911	49.453338
924.146092	47.941194	49.458343
920.534086	52.341045	49.463348
917.010904	58.650588	49.468353
913.522726	59.187297	49.473357
910.487133	54.794146	49.478362
906.765232	54.883195	49.483367
903.127799	47.091032	49.488372
899.205296	54.557367	49.493377
895.916932	53.626664	49.498381
892.816238	52.625621	49.503386
889.312007	50.409270	49.508391
886.000755	52.560389	49.513396
882.243392	54.796771	49.518401
878.566257	52.882576	49.523405
875.060925	44.335883	49.528410
871.088841	54.419969	49.533415
867.989511	48.882005	49.538420
864.780465	51.877736	49.543425
861.375680	50.060350	49.548429
857.643913	48.923435	49.553434
853.652882	58.238537	49.558439
850.213932	43.623076	49.563444
846.965223	59.203756	49.568449
843.521289	55.864410	49.573453
839.948976	45.955115	49.578458
836.511874	48.549761	49.583463
833.023922	45.653858	49.588468
829.685883	48.419741	49.593473
826.027057	53.981630	49.598477
823.026379	45.653775	49.603482
819.385777	48.988764	49.608487
815.573981	51.012169	49.613492
812.002072	44.313948	49.618497
808.593513	58.954590	49.623501
804.951911	43.747442	49.628506
801.370489	48.718331	49.633511
798.065603	43.867259	49.638516
794.570074	49.093689	49.643521
790.871420	48.530582	49.648525
787.628499	45.659815	49.653530
783.909626	55.479869	49.658535
780.673591	48.523727	49.663540
777.118256	44.983441	49.668545
773.279442	49.567305	49.673549
769.887776	41.638838	49.678554
766.222307	50.656495	49.683559
763.072289	49.384742	49.688564
759.299970	51.794304	49.693569
756.031428	47.674715	49.698573
752.693279	39.712613	49.703578
748.922184	46.304357	49.708583
745.132032	33.762025	49.713588
742.418204	45.089711	49.718593
738.433332	49.949408	49.723597
735.381213	36.896727	49.728602
731.341382	47.712680	49.733607
727.884189	40.955489	49.738612
724.660999	37.227471	49.743617
720.922793	40.795956	49.748621
717.234806	42.932972	49.753626
713.713391	44.113940	49.758631
710.434510	45.633630	49.763636
706.737722	40.618960	49.768641
703.096578	50.607244	49.773645
700.055316	48.097392	49.778650
696.471389	50.271995	49.783655
693.078253	49.215263	49.788660
689.403183	45.469009	49.793665
685.780184	48.601960	49.798669
682.796079	42.334265	49.803674
678.796775	51.176111	49.808679
675.008029	46.039723	49.813684
671.745400	35.680474	49.818689
668.360287	41.990680	49.823693
664.839773	44.190215	49.828698
661.425878	47.065996	49.833703
657.853609	46.669889	49.838708
654.768165	52.920795	49.843713
650.997084	52.698003	49.848717
647.514477	45.448086	49.853722
643.521361	51.292977	49.858727
640.233879	45.496447	49.863732
636.895521	45.313859	49.868737
633.294104	45.453789	49.873741
629.957590	47.191261	49.878746
626.260333	46.567849	49.883751
622.847447	45.112415	49.888756
619.632656	47.789531	49.893761
615.848109	40.618263	49.898765
612.182103	44.185011	49.903770
608.334330	56.565565	49.908775
605.197608	45.563481	49.913780
601.999786	49.247168	49.918785
598.335425	45.315769	49.923789
594.996968	40.957162	49.928794
591.883999	51.821819	49.933799
587.668001	41.117468	49.938804
584.066558	41.611739	49.943809
580.768875	50.904336	49.948813
577.474145	51.183186	49.953818
573.758844	53.188435	49.958823
570.340432	42.489633	49.963828
567.055457	45.513028	49.968833
563.193958	51.463984	49.973837
560.015520	42.445698	49.978842
556.397860	49.975328	49.983847
552.747035	51.385264	49.988852
548.941839	46.004693	49.993857
545.541864	43.107792	49.998861
542.039086	37.427054	50.003866
539.021249	54.468196	50.008871
535.564516	52.484940	50.013876
531.841415	46.126674	50.018881
528.129892	45.097384	50.023885
524.814636	44.395536	50.028890
521.177611	55.885931	50.033895
518.024188	52.953814	50.038900
514.318400	39.904869	50.043905
510.577494	51.288050	50.048909
506.953127	42.712509	50.053914
503.393039	45.047932	50.058919
500.491139	37.071747	50.063924
497.378183	31.804881	50.068929
493.182236	43.464537	50.073933
489.999344	46.921288	50.078938
486.054609	53.435688	50.083943
482.630369	43.724876	50.088948
479.219864	43.800305	50.093953
475.468214	47.532257	50.098957
472.097044	39.379202	50.103962
468.401806	44.541839	50.108967
465.041575	33.001966	50.113972
462.057279	43.713716	50.118977
457.956235	51.888066	50.123981
455.120802	44.762054	50.128986
451.539577	49.622215	50.133991
448.139863	42.081031	50.138996
444.136296	45.399801	50.144001
440.704552	47.234375	50.149005
437.567109	42.629369	50.154010
433.559138	46.176610	50.159015
429.903557	51.171732	50.164020
426.441394	47.604343	50.169025
422.934909	48.678621	50.174029
419.675737	46.465315	50.179034
416.372003	56.448543	50.184039
412.863352	46.336446	50.189044
409.321199	53.572767	50.194049
405.617546	46.828695	50.199053
402.211884	45.277258	50.204058
398.591830	58.286738	50.209063
395.156968	47.577879	50.214068
391.797168	47.360696	50.219073
388.000788	49.081206	50.224077
384.588274	42.756873	50.229082
381.068633	47.404978	50.234087
377.490034	38.793868	50.239092
374.105918	40.190777	50.244097
370.547594	38.485947	50.249101
367.407484	45.770405	50.254106
363.664004	45.834415	50.259111
360.186663	47.090820	50.264116
356.621575	42.691606	50.269121
352.848486	46.398436	50.274125
349.412827	45.338881	50.279130
346.072153	52.857042	50.284135
342.643714	46.607959	50.289140
339.186181	48.256740	50.294145
335.414931	50.893970	50.299149
332.153575	44.403749	50.304154
328.522617	57.804058	50.309159
324.977499	52.164747	50.314164
321.764447	39.073941	50.319169
318.169990	44.205084	50.324173
314.757477	40.120637	50.329178
311.060438	50.139788	50.334183
307.622757	39.377610	50.339188
303.884560	42.335554	50.344193
300.026839	49.004097	50.349197
297.058473	44.493011	50.354202
293.248314	46.595317	50.359207
290.225658	49.008443	50.364212
286.897426	37.969812	50.369217
283.319581	42.266330	50.374221
279.351517	32.836381	50.379226
275.726156	40.449482	50.384231
272.027298	45.517793	50.389236
269.209730	43.261068	50.394241
265.363981	38.731566	50.399245
261.999717	34.573180	50.404250
258.531330	48.156976	50.409255
255.482906	43.582432	50.414260
251.728600	39.177897	50.419265
247.698162	46.445956	50.424269
244.235146	32.220374	50.429274
241.037882	36.337425	50.434279
237.553382	30.372334	50.439284
234.275231	38.690659	50.444289
230.214103	43.321844	50.449293
227.022043	38.782324	50.454298
223.334229	40.773845	50.459303
219.823863	37.017851	50.464308
216.696248	30.839019	50.469313
213.034015	39.087432	50.474317
209.982037	41.343784	50.479322
206.365621	44.814275	50.484327
202.367674	43.440499	50.489332
198.906889	37.743795	50.494337
195.212268	40.492494	50.499341
191.848614	35.846823	50.504346
188.128334	39.599232	50.509351
184.584526	37.778280	50.514356
181.403818	40.766499	50.519361
178.068477	48.989335	50.524365
174.766192	38.797713	50.529370
170.824018	40.993353	50.534375
167.675280	43.720340	50.539380
163.901088	38.357167	50.544385
160.228454	40.909464	50.549389
156.830494	36.661433	50.554394
153.313118	42.062157	50.559399
149.985518	37.489970	50.564404
146.279541	34.827432	50.569409
142.380875	41.606764	50.574413
138.974118	43.798141	50.579418
135.580337	48.015400	50.584423
132.926382	42.870113	50.589428
129.418142	46.943847	50.594433
125.612459	42.857372	50.599437
122.036531	36.656608	50.604442
118.249105	38.986345	50.609447
114.546996	45.880607	50.614452
111.357315	35.706270	50.619457
107.616934	36.494313	50.624461
104.692695	45.213112	50.629466
101.359136	42.460962	50.634471
97.188393	40.974908	50.639476
93.818353	43.318756	50.644481
90.091270	45.616957	50.649485
87.173383	41.521975	50.654490
83.320591	42.283233	50.659495
79.647420	42.345830	50.664500
76.601900	37.416536	50.669505
72.427014	49.579129	50.674509
68.903085	39.472658	50.679514
65.680294	41.559473	50.684519
62.444525	39.934182	50.689524
58.952445	41.037902	50.694529
55.316169	49.639784	50.699533
51.547909	37.477021	50.704538
48.082022	36.925239	50.709543
44.833560	42.005703	50.714548
41.815782	38.600140	50.719553
37.955406	49.286960	50.724557
34.415786	38.635629	50.729562
30.915296	48.159139	50.734567
27.178922	38.076264	50.739572
23.573531	43.936780	50.744577
19.810919	44.427751	50.749581
16.696817	36.585933	50.754586
13.604306	41.771829	50.759591
9.871074	45.140312	50.764596
6.051981	45.855207	50.769601
2.352088	40.657663	50.774605