Fri Aug 26 13:27:28 2022

Number of Points = 9930

Depth (nm)	Load (N)	Time (s)
1.021420	109.666129	0.000000
0.675597	106.328348	0.005005
0.827130	93.675269	0.010010
0.405418	82.952694	0.015014
-0.231769	74.108081	0.020019
-0.023440	71.250320	0.025024
-0.600427	70.966656	0.030029
-0.792012	59.059863	0.035034
-0.965140	50.725120	0.040038
-1.712739	42.501970	0.045043
-1.750789	25.781541	0.050048
-2.152165	32.237560	0.055053
-2.366717	22.567897	0.060058
-2.873830	23.285719	0.065062
-2.998431	10.656711	0.070067
-3.072513	3.451805	0.075072
-3.621217	-6.254398	0.080077
-3.906750	-0.771844	0.085082
-3.932646	6.185667	0.090086
-4.167004	0.144626	0.095091
-4.573046	-10.406331	0.100096
-4.877078	-15.693066	0.105101
-4.860767	-19.033424	0.110106
-5.189223	-16.170005	0.115110
-5.929065	-11.170356	0.120115
-6.014036	-15.016945	0.125120
-6.307457	-17.742789	0.130125
-6.451515	-9.662779	0.135130
-6.522688	-16.469512	0.140134
-7.318574	-8.832159	0.145139
-7.767717	-14.352554	0.150144
-8.116884	-11.827582	0.155149
-8.097721	-12.090172	0.160154
-8.046125	-15.097516	0.165158
-8.004344	-12.184178	0.170163
-7.924655	-15.686259	0.175168
-8.175252	-4.875264	0.180173
-9.058695	-0.542925	0.185178
-8.845884	-14.527867	0.190182
-9.163182	-12.545674	0.195187
-9.902924	-4.287497	0.200192
-10.207915	-13.209097	0.205197
-10.587035	-15.244581	0.210202
-10.466856	-19.613473	0.215206
-10.635663	-3.370603	0.220211
-10.866898	-12.857322	0.225216
-11.650336	-17.012760	0.230221
-11.790266	-6.472087	0.235226
-11.774068	-3.589565	0.240230
-12.471067	3.598980	0.245235
-12.034640	-4.371916	0.250240
-12.108745	-1.029261	0.255245
-12.843174	-6.372367	0.260250
-13.114341	-7.747643	0.265254
-13.474179	-1.854904	0.270259
-13.480244	-3.711200	0.275264
-13.834335	-11.454611	0.280269
-13.613695	-3.190945	0.285274
-13.901025	-11.865368	0.290278
-14.537641	-1.835795	0.295283
-15.080539	-7.664285	0.300288
-15.103258	-2.561161	0.305293
-15.164161	7.154162	0.310298
-14.913011	-8.336315	0.315302
-15.805433	3.305414	0.320307
-15.823782	-5.471000	0.325312
-16.159122	-2.084508	0.330317
-16.320897	-5.678704	0.335322
-16.902191	-7.103767	0.340326
-17.543372	-2.489621	0.345331
-17.337703	-6.277064	0.350336
-17.918822	-5.047866	0.355341
-17.683213	-3.600994	0.360346
-17.721018	-19.302726	0.365350
-18.212727	-7.970158	0.370355
-18.428678	-14.593004	0.375360
-18.795546	-4.257433	0.380365
-19.301034	-6.488370	0.385370
-19.507530	-7.383351	0.390374
-19.255627	-3.828874	0.395379
-19.239223	-9.712809	0.400384
-20.202628	1.924153	0.405389
-20.530220	3.325841	0.410394
-20.494327	-4.054365	0.415398
-20.727959	-0.582472	0.420403
-20.759740	-6.699342	0.425408
-21.296517	-13.167836	0.430413
-21.916759	0.146201	0.435418
-22.007590	-14.455825	0.440422
-21.997997	9.130539	0.445427
-22.026894	9.884631	0.450432
-22.301734	-3.821918	0.455437
-22.979559	-4.064570	0.460442
-23.008878	0.103147	0.465446
-23.855317	6.172888	0.470451
-23.615774	-6.901929	0.475456
-23.678383	-1.482558	0.480461
-23.773623	-6.194385	0.485466
-24.052724	-4.306721	0.490470
-25.175392	9.120349	0.495475
-25.135282	-3.265383	0.500480
-25.152340	-0.915500	0.505485
-25.463164	-2.831910	0.510490
-25.550972	-2.916500	0.515494
-25.324237	-2.588172	0.520499
-25.853692	-9.111590	0.525504
-26.238015	-10.959610	0.530509
-26.524741	-11.807300	0.535514
-26.297355	-6.572282	0.540518
-26.737050	-3.697869	0.545523
-27.247961	-18.386340	0.550528
-27.576453	-6.591985	0.555533
-27.807542	-1.978417	0.560538
-27.740606	-15.972279	0.565542
-28.436643	-3.956187	0.570547
-28.985767	-10.318360	0.575552
-29.613653	-0.087674	0.580557
-29.556389	-0.735832	0.585562
-29.584244	-9.346254	0.590566
-29.755125	-7.984784	0.595571
-29.760364	-8.923756	0.600576
-29.849523	-10.156533	0.605581
-29.862428	-4.545593	0.610586
-29.658736	-14.900425	0.615590
-30.493022	-0.309756	0.620595
-30.797701	-7.858388	0.625600
-31.398611	-4.876620	0.630605
-32.298038	-4.774733	0.635610
-32.090140	-7.910814	0.640614
-32.498196	-5.319727	0.645619
-32.690231	-10.908626	0.650624
-32.606249	-3.310192	0.655629
-32.862285	-1.049646	0.660634
-32.628823	-8.625120	0.665638
-32.717955	2.942155	0.670643
-33.225894	-2.879123	0.675648
-33.700742	-2.273889	0.680653
-34.337140	2.738131	0.685658
-34.014906	-3.117495	0.690662
-34.976992	0.673453	0.695667
-35.272952	-10.163550	0.700672
-35.327976	-0.202385	0.705677
-35.755304	-6.599340	0.710682
-34.926553	-8.582451	0.715686
-35.594897	-4.995421	0.720691
-35.727054	-9.752117	0.725696
-36.502266	-9.381679	0.730701
-36.701588	-1.030482	0.735706
-36.779144	-2.331502	0.740710
-37.005725	-1.787068	0.745715
-37.209266	-7.269776	0.750720
-37.717351	-3.780461	0.755725
-38.020367	2.714013	0.760730
-38.464050	-9.299007	0.765734
-38.657670	2.645190	0.770739
-38.503155	-2.538941	0.775744
-38.646774	-4.500366	0.780749
-38.664165	-1.052651	0.785754
-39.041360	4.738393	0.790758
-39.827591	5.971055	0.795763
-39.953254	-0.846180	0.800768
-39.962338	-1.376444	0.805773
-40.210236	6.257848	0.810778
-40.388288	-13.357610	0.815782
-41.630649	-8.150010	0.820787
-41.615732	-6.994632	0.825792
-41.408170	-5.410522	0.830797
-41.819338	-7.906070	0.835802
-41.564609	-9.847262	0.840806
-41.908742	-5.061077	0.845811
-41.612285	-8.005310	0.850816
-42.569226	-3.291383	0.855821
-43.178125	-11.241882	0.860826
-42.980507	-16.543447	0.865830
-42.925866	1.110411	0.870835
-43.543083	-11.619041	0.875840
-44.158893	-9.169607	0.880845
-44.178911	-9.891151	0.885850
-44.329440	-10.443683	0.890854
-44.506551	-7.306446	0.895859
-44.344201	-9.752090	0.900864
-45.113887	-1.517724	0.905869
-45.824342	-9.155030	0.910874
-45.787523	-7.901826	0.915878
-46.065015	-5.527213	0.920883
-45.922258	-8.194424	0.925888
-45.898839	-4.126665	0.930893
-46.815274	-8.422741	0.935898
-46.859874	-9.023402	0.940902
-47.363557	-2.937432	0.945907
-47.506523	-7.904408	0.950912
-47.252641	-5.811838	0.955917
-47.717472	-7.394232	0.960922
-48.515727	-4.103338	0.965926
-49.122497	-2.354473	0.970931
-49.028346	-3.973283	0.975936
-48.542416	-5.748000	0.980941
-48.995238	-4.358450	0.985946
-48.746817	-9.766000	0.990950
-49.361120	-1.087610	0.995955
-49.760675	-5.144637	1.000960
-50.050842	-5.251501	1.005965
-49.879551	-6.312867	1.010970
-50.096548	-14.624927	1.015974
-50.880281	-5.236814	1.020979
-51.275665	-12.704883	1.025984
-51.426678	-15.063773	1.030989
-51.874566	-10.679034	1.035994
-51.383673	-13.827539	1.040998
-52.588827	-9.435622	1.046003
-52.737470	-12.462406	1.051008
-53.014523	-10.091026	1.056013
-53.100368	-11.077556	1.061018
-53.303998	-11.637638	1.066022
-53.198143	-5.614937	1.071027
-53.340465	-16.785890	1.076032
-53.376180	-20.162437	1.081037
-54.224937	-15.402086	1.086042
-54.352480	-20.580259	1.091046
-54.754819	-10.270807	1.096051
-54.551458	-9.306115	1.101056
-54.609156	-13.903566	1.106061
-55.634718	-11.874370	1.111066
-55.688967	-14.586833	1.116070
-55.926369	1.005516	1.121075
-55.961084	-13.791898	1.126080
-56.543267	-6.776254	1.131085
-57.503397	-11.381888	1.136090
-57.223776	-5.114170	1.141094
-56.698218	-2.238192	1.146099
-57.077395	-11.258964	1.151104
-57.352503	-12.763333	1.156109
-57.780511	-7.638236	1.161114
-58.173586	-25.477038	1.166118
-58.773461	-14.757198	1.171123
-58.909349	-10.522273	1.176128
-59.215596	-13.774446	1.181133
-59.485048	-13.308754	1.186138
-58.954428	-16.713371	1.191142
-59.436372	2.064865	1.196147
-59.318036	-16.881752	1.201152
-60.126744	-14.861011	1.206157
-60.260626	-12.492941	1.211162
-60.400257	-9.975285	1.216166
-60.931759	-17.564521	1.221171
-61.405223	-19.161388	1.226176
-61.964505	-12.301166	1.231181
-62.028608	-5.796440	1.236186
-61.660196	-10.517182	1.241190
-62.323463	-9.831992	1.246195
-62.012642	-9.016904	1.251200
-62.140482	-3.097016	1.256205
-62.675514	-10.040325	1.261210
-62.976646	-7.450068	1.266214
-63.256112	-0.864354	1.271219
-63.576797	-1.567556	1.276224
-63.875583	-5.165727	1.281229
-64.652712	-4.377391	1.286234
-64.371121	-11.065048	1.291238
-64.627781	-0.620092	1.296243
-65.132617	0.369448	1.301248
-64.595880	-8.661059	1.306253
-65.675891	-2.773246	1.311258
-66.038155	-8.107857	1.316262
-66.463665	-3.229911	1.321267
-66.312290	-3.247341	1.326272
-66.377273	-13.610957	1.331277
-66.325507	-7.567181	1.336282
-66.286996	-16.130984	1.341286
-66.577456	-0.609467	1.346291
-67.309088	-3.637227	1.351296
-67.240026	-10.987792	1.356301
-68.050364	-5.423530	1.361306
-68.409220	-1.505051	1.366310
-69.006485	-4.294314	1.371315
-68.657101	-5.462500	1.376320
-68.977543	-6.418830	1.381325
-69.180830	-5.704022	1.386330
-68.753385	-3.676440	1.391334
-69.704280	-3.076175	1.396339
-70.292266	-10.280147	1.401344
-70.300962	-9.443783	1.406349
-70.671247	-6.213197	1.411354
-70.551228	-10.980682	1.416358
-70.596403	-7.851334	1.421363
-71.130640	-11.624807	1.426368
-71.848485	-8.143961	1.431373
-71.926483	-5.534664	1.436378
-71.861750	-5.728422	1.441382
-71.814061	-6.954034	1.446387
-71.970300	-16.601112	1.451392
-72.512769	-6.045223	1.456397
-73.196138	-12.190345	1.461402
-72.912846	-8.387668	1.466406
-73.119784	-9.782433	1.471411
-73.450557	0.085627	1.476416
-73.592332	-2.511974	1.481421
-74.351145	-1.444926	1.486426
-74.239899	-13.509541	1.491430
-74.502525	-8.666448	1.496435
-75.211862	1.592736	1.501440
-75.653681	-16.972445	1.506445
-76.064330	-4.943847	1.511450
-75.972664	-13.395710	1.516454
-76.282333	0.312874	1.521459
-76.365460	-7.371486	1.526464
-76.240326	-9.314645	1.531469
-76.254440	-2.779739	1.536474
-76.225301	-14.015352	1.541478
-77.211696	-6.579282	1.546483
-77.301323	-3.620176	1.551488
-77.465361	2.340150	1.556493
-77.959969	3.926024	1.561498
-78.662294	-12.447330	1.566502
-78.890082	0.460762	1.571507
-78.982284	-0.850633	1.576512
-78.895049	-1.728075	1.581517
-79.290523	-4.618356	1.586522
-79.008358	-13.352970	1.591526
-79.616814	-3.115823	1.596531
-79.653711	-8.399857	1.601536
-79.983654	-5.520388	1.606541
-80.825999	-10.995376	1.611546
-80.931398	-10.963335	1.616550
-80.723388	-11.644455	1.621555
-80.999571	-11.361206	1.626560
-81.329013	-9.908612	1.631565
-82.074287	-5.237134	1.636570
-82.193496	-10.558969	1.641574
-82.070213	-8.164503	1.646579
-82.179886	-8.362743	1.651584
-82.411190	-8.542044	1.656589
-83.271876	-11.786980	1.661594
-83.413307	-10.347841	1.666598
-83.644343	-6.993410	1.671603
-83.727819	-5.838530	1.676608
-83.746461	-18.297353	1.681613
-83.749682	-6.354339	1.686618
-84.293376	-18.763046	1.691622
-84.927151	-17.164996	1.696627
-85.243023	-4.939193	1.701632
-84.804815	-9.091857	1.706637
-85.622289	-8.167530	1.711642
-85.746409	-9.657444	1.716646
-85.915347	-8.229841	1.721651
-86.406058	-10.327039	1.726656
-86.266013	-8.700782	1.731661
-86.703857	-10.325339	1.736666
-86.680268	-14.745627	1.741670
-87.382620	-6.164259	1.746675
-87.876221	-3.755998	1.751680
-87.836133	-3.490356	1.756685
-87.852355	0.624702	1.761690
-87.664947	-9.186612	1.766694
-88.270535	-9.769527	1.771699
-89.139249	-4.828902	1.776704
-89.386087	-7.539853	1.781709
-89.583890	-4.475322	1.786714
-89.302818	-8.056212	1.791718
-89.753373	-8.226685	1.796723
-89.643542	-1.420023	1.801728
-89.694142	-9.913008	1.806733
-90.544680	0.656050	1.811738
-90.595133	-4.704964	1.816742
-90.866954	-1.983235	1.821747
-91.080796	-7.091028	1.826752
-91.606468	-12.251503	1.831757
-92.021141	-6.666593	1.836762
-92.444021	-8.217554	1.841766
-92.490085	5.051371	1.846771
-92.826555	-4.880849	1.851776
-92.509801	-9.391075	1.856781
-92.576055	-8.200914	1.861786
-92.524936	-6.658883	1.866790
-93.276288	-4.520525	1.871795
-93.892701	-9.540328	1.876800
-93.663463	-15.235941	1.881805
-94.346560	-19.846741	1.886810
-95.043178	-11.329541	1.891814
-95.410714	-5.366007	1.896819
-95.027482	-3.670050	1.901824
-95.225255	-12.431172	1.906829
-95.570513	-8.201613	1.911834
-95.430595	-11.902888	1.916838
-95.761473	-5.815353	1.921843
-96.110152	8.683890	1.926848
-96.478631	0.262540	1.931853
-97.096025	4.506001	1.936858
-97.197706	1.617431	1.941862
-97.126427	4.586285	1.946867
-97.369517	7.673687	1.951872
-97.418458	-2.420357	1.956877
-98.135828	0.307473	1.961882
-98.150236	-7.555258	1.966886
-98.288577	-6.708199	1.971891
-98.424298	-12.600079	1.976896
-98.638522	-2.367370	1.981901
-99.785312	-6.203650	1.986906
-99.597851	-14.429989	1.991910
-99.607476	-5.738190	1.996915
-99.832061	-10.523313	2.006912
-100.010083	-8.753747	2.016909
-99.291817	-7.136405	2.026906
-98.374622	-14.273827	2.036902
-98.504388	-15.118775	2.046899
-98.181851	-9.882514	2.056896
-97.167532	-1.804850	2.066893
-96.886458	-6.895106	2.076890
-95.937835	-5.687417	2.086886
-95.885270	-6.747648	2.096883
-95.607270	-11.045504	2.106880
-94.752832	-0.896625	2.116877
-94.394253	-2.343444	2.126874
-93.486677	-8.202796	2.136870
-93.324391	-11.529163	2.146867
-93.012892	-10.355316	2.156864
-91.812843	-13.726059	2.166861
-91.968830	-6.730084	2.176858
-91.601398	-3.148004	2.186854
-90.485804	-8.672293	2.196851
-90.444056	-4.817766	2.206848
-89.754669	-2.828476	2.216845
-89.207189	-7.732138	2.226842
-88.871277	-9.919833	2.236838
-87.705532	-4.444239	2.246835
-87.664758	-7.000947	2.256832
-87.783943	-10.372185	2.266829
-87.121018	-3.462533	2.276826
-86.287100	-9.867927	2.286822
-85.359158	-5.140891	2.296819
-85.247997	-6.970489	2.306816
-85.038829	-0.709250	2.316813
-84.016362	-4.283586	2.326810
-83.357993	-3.458340	2.336806
-83.457388	-6.534898	2.346803
-82.962492	-8.931072	2.356800
-82.622210	-1.613236	2.366797
-81.553963	2.116310	2.376794
-80.968255	1.631946	2.386790
-80.796597	2.308068	2.396787
-80.132368	-4.704444	2.406784
-79.416026	-3.805864	2.416781
-78.856734	-1.400357	2.426778
-79.015085	-5.563754	2.436774
-78.526462	-4.826115	2.446771
-78.054955	-3.727863	2.456768
-77.184232	-6.264913	2.466765
-76.515025	-0.265362	2.476762
-76.335138	1.328106	2.486758
-75.360756	-6.540455	2.496755
-74.971874	-2.267992	2.506752
-75.058699	-1.120819	2.516749
-74.478964	1.161134	2.526746
-73.936729	1.260057	2.536742
-73.149134	1.637546	2.546739
-72.537620	-0.235113	2.556736
-72.534373	-3.204114	2.566733
-71.471487	-6.648532	2.576730
-70.779230	-7.687991	2.586726
-70.622266	-9.980867	2.596723
-70.801062	-10.574270	2.606720
-69.600115	-8.170471	2.616717
-69.218382	-6.516567	2.626714
-68.068798	-2.140807	2.636710
-68.083209	-5.385814	2.646707
-67.780531	-5.781762	2.656704
-67.637692	0.024157	2.666701
-66.646738	1.342462	2.676698
-66.347404	-2.011582	2.686694
-65.485014	-3.641378	2.696691
-65.237176	-10.779117	2.706688
-64.729374	-6.300265	2.716685
-64.359661	-7.603104	2.726682
-63.874535	-3.225254	2.736678
-63.105409	-5.708474	2.746675
-62.748499	-5.197406	2.756672
-62.186147	-11.174060	2.766669
-61.133365	-7.160182	2.776666
-60.983738	-5.698213	2.786662
-61.238623	-7.230074	2.796659
-60.438618	-7.766810	2.806656
-59.947722	-4.188113	2.816653
-59.005879	-5.133390	2.826650
-58.661735	-14.455985	2.836646
-58.323258	-13.517578	2.846643
-57.246603	-15.608371	2.856640
-57.049692	-5.353945	2.866637
-56.888761	-8.483707	2.876634
-55.994875	-14.264901	2.886630
-55.336251	-15.254775	2.896627
-55.436424	-15.949115	2.906624
-55.044819	-5.889723	2.916621
-53.866705	-9.082828	2.926618
-53.549547	-6.015587	2.936614
-53.443440	-4.990317	2.946611
-52.907771	-12.223554	2.956608
-52.197401	-10.541627	2.966605
-51.343546	-8.695147	2.976602
-51.415130	-11.462434	2.986598
-50.320607	-8.253311	2.996595
-49.963550	-9.490826	3.006592
-49.787636	-6.547306	3.016589
-49.370766	-6.682278	3.026586
-48.455730	-1.728323	3.036582
-48.329163	-5.806208	3.046579
-47.573895	-14.328038	3.056576
-47.306649	-5.766601	3.066573
-46.684302	-10.697759	3.076570
-45.902339	-10.838892	3.086566
-45.860559	-8.311628	3.096563
-45.208481	-8.362849	3.106560
-44.361838	-7.899523	3.116557
-43.933902	-10.842784	3.126554
-43.876651	-13.953234	3.136550
-42.909105	-5.244250	3.146547
-42.462809	-7.800745	3.156544
-42.315488	-2.340800	3.166541
-41.591269	-4.259516	3.176538
-41.045134	-11.557737	3.186534
-40.882632	-5.362087	3.196531
-40.042412	-10.457043	3.206528
-39.895000	-8.820506	3.216525
-39.026139	-6.640587	3.226522
-38.407677	-8.036007	3.236518
-38.379357	-9.466250	3.246515
-37.189467	-11.128030	3.256512
-36.857641	-9.890824	3.266509
-36.952658	-9.550136	3.276506
-36.291928	-11.617350	3.286502
-35.635316	-7.373900	3.296499
-35.176407	-7.673801	3.306496
-34.382895	-3.581540	3.316493
-34.265765	-7.638949	3.326490
-33.748620	-5.166692	3.336486
-33.012376	-5.120148	3.346483
-32.636041	-6.246629	3.356480
-32.192262	-4.364808	3.366477
-31.314375	-7.083531	3.376474
-31.268248	-17.104131	3.386470
-30.866258	-10.343911	3.396467
-29.906190	-7.348260	3.406464
-29.666427	-7.249757	3.416461
-28.914780	-9.027029	3.426458
-28.151811	-13.495425	3.436454
-28.136994	-17.726963	3.446451
-27.762194	-11.260272	3.456448
-26.985383	-13.165001	3.466445
-26.789106	-12.730288	3.476442
-25.982234	-12.770765	3.486438
-25.162915	-18.610037	3.496435
-24.999595	-15.952817	3.506432
-24.928881	-14.880856	3.516429
-24.236036	-13.753711	3.526426
-23.740425	-6.548752	3.536422
-22.873710	-11.508454	3.546419
-22.413786	-10.988084	3.556416
-22.534836	-10.494460	3.566413
-21.669397	-4.313224	3.576410
-21.360545	-16.265838	3.586406
-19.991011	-9.190612	3.596403
-19.578580	-11.254011	3.606400
-19.390493	-10.722992	3.616397
-19.382359	-6.948758	3.626394
-18.960839	-10.888840	3.636390
-18.463218	-8.103109	3.646387
-17.422668	-7.023765	3.656384
-16.938288	-6.703598	3.666381
-16.957282	-6.365243	3.676378
-15.840783	-7.892056	3.686374
-15.431949	-11.966373	3.696371
-15.218892	-11.394895	3.706368
-14.127660	-9.338293	3.716365
-14.045468	-8.264951	3.726362
-13.909600	-6.661460	3.736358
-12.819920	-11.994820	3.746355
-12.437711	-11.706260	3.756352
-12.407032	-17.631810	3.766349
-11.498553	-19.797783	3.776346
-11.288791	-15.845876	3.786342
-10.193921	-10.080484	3.796339
-9.692767	-10.456651	3.806336
-9.717547	-11.631547	3.816333
-9.262156	-19.568181	3.826330
-8.323143	-13.493432	3.836326
-8.293297	-9.817609	3.846323
-7.234699	-8.902626	3.856320
-6.646874	-11.873949	3.866317
-6.654860	-14.252011	3.876314
-6.611100	-4.943046	3.886310
-5.622786	-4.143827	3.896307
-5.049835	-3.739252	3.906304
-4.958512	2.673385	3.916301
-4.285252	11.801988	3.926298
-3.611652	20.468060	3.936294
-3.394839	18.058161	3.946291
-3.298855	32.953152	3.956288
-2.507443	51.164157	3.966285
-1.650277	66.352464	3.976282
-1.237473	71.346627	3.986278
-0.945911	81.599042	3.996275
-0.254135	94.906169	4.006272
-0.149086	102.827699	4.016269
0.000000	114.722902	4.021274
0.835302	122.232886	4.026278
0.650587	118.645399	4.031283
0.674277	129.467553	4.036288
1.041605	133.371071	4.041293
1.541996	143.419844	4.046298
1.136343	139.344749	4.051302
1.138775	133.988108	4.056307
1.130371	147.947292	4.061312
1.611252	139.605589	4.066317
1.409130	145.768042	4.071322
1.318911	129.058803	4.076326
1.543830	132.870602	4.081331
1.369426	132.438837	4.086336
1.094534	131.402642	4.091341
1.443479	133.512065	4.096346
1.419174	133.430242	4.101350
1.475876	133.282024	4.106355
1.172787	133.158188	4.111360
1.513287	145.946276	4.116365
1.859540	141.232107	4.121370
1.400317	130.331851	4.126374
1.392312	120.784995	4.131379
1.011482	119.119908	4.136384
1.431892	138.108968	4.141389
1.589194	141.339693	4.146394
1.339771	135.421170	4.151398
1.824929	145.092677	4.156403
1.632632	143.170450	4.161408
1.633326	135.504609	4.166413
0.988246	140.290235	4.171418
1.445829	139.342469	4.176422
1.577969	142.127872	4.181427
1.503839	146.369038	4.186432
1.777411	147.560083	4.191437
1.764758	145.809197	4.196442
1.868066	140.066700	4.201446
1.852594	151.451769	4.206451
1.473104	143.677443	4.211456
1.712601	147.467994	4.216461
1.903026	152.575942	4.221466
1.461568	150.917128	4.226470
1.416387	142.458020	4.231475
1.717568	148.842659	4.236480
1.760846	143.410056	4.241485
1.995937	147.444894	4.246490
1.926796	148.347623	4.251494
1.996342	149.288868	4.256499
1.668795	138.096032	4.261504
1.653221	150.328976	4.266509
1.963263	148.201990	4.271514
2.043581	148.379116	4.276518
2.061703	142.918793	4.281523
1.675921	137.445430	4.286528
1.676844	117.539371	4.291533
1.957837	139.878304	4.296538
1.765389	139.971353	4.301542
1.792822	139.881474	4.306547
1.822264	153.553204	4.311552
2.182813	153.237459	4.316557
2.159427	158.600154	4.321562
2.082030	145.166457	4.326566
1.485166	136.204807	4.331571
2.066474	152.157028	4.336576
2.179897	145.248728	4.341581
1.659165	148.113636	4.346586
2.015831	146.994926	4.351590
2.366901	156.212767	4.356595
2.184678	135.427232	4.361600
1.896718	135.462387	4.366605
1.934836	136.493944	4.371610
2.052820	144.884391	4.376614
2.229332	140.544652	4.381619
2.107731	135.188341	4.386624
2.012806	142.030107	4.391629
1.814586	145.955246	4.396634
1.815795	150.969271	4.401638
2.445110	145.888335	4.406643
2.078797	156.957884	4.411648
2.217912	150.934570	4.416653
2.133819	150.466598	4.421658
1.999087	151.661105	4.426662
2.264941	143.441462	4.431667
2.048978	158.002429	4.436672
2.159314	148.914845	4.441677
2.099445	150.768392	4.446682
2.026445	151.247791	4.451686
2.013760	150.417534	4.456691
1.978427	157.610686	4.461696
2.693580	147.944894	4.466701
2.297659	145.608295	4.471706
2.131625	148.784962	4.476710
2.384489	145.980365	4.481715
2.380325	146.958396	4.486720
2.720035	142.052262	4.491725
2.211591	147.329129	4.496730
2.271146	151.973413	4.501734
2.382248	150.994173	4.506739
2.150897	154.130393	4.511744
2.281840	139.816401	4.516749
2.240668	140.050406	4.521754
2.588435	147.949512	4.526758
2.069609	141.215580	4.531763
2.153892	151.028596	4.536768
2.618365	164.800276	4.541773
2.512853	161.323831	4.546778
2.799566	166.226972	4.551782
2.996503	154.243804	4.556787
2.585521	152.466353	4.561792
2.291284	149.414753	4.566797
2.427436	140.535118	4.571802
2.586941	140.649297	4.576806
2.459102	137.698337	4.581811
2.499074	148.517967	4.586816
2.810127	163.009538	4.591821
2.646136	152.673889	4.596826
2.477675	154.275432	4.601830
2.449063	157.452852	4.606835
2.447357	171.939342	4.611840
2.536221	160.808204	4.616845
2.665773	171.772085	4.621850
2.848974	170.335542	4.626854
3.092783	166.361795	4.631859
2.620914	176.248762	4.636864
2.828072	163.745156	4.641869
2.930910	172.653652	4.646874
2.843850	172.119704	4.651878
2.834474	160.386947	4.656883
2.386762	157.735717	4.661888
2.304931	165.594152	4.666893
2.348693	173.119834	4.671898
2.860564	169.857303	4.676902
2.927318	173.598827	4.681907
2.472311	173.112677	4.686912
2.789359	174.970815	4.691917
2.766112	173.844817	4.696922
2.703878	163.287681	4.701926
2.638804	167.195258	4.706931
2.619890	172.183949	4.711936
3.089783	176.615658	4.716941
2.946673	172.929936	4.721946
2.829243	163.513985	4.726950
3.237130	164.712592	4.731955
2.760711	166.988490	4.736960
2.758475	164.755103	4.741965
2.968987	174.678190	4.746970
3.454242	178.164736	4.751974
3.111304	168.401090	4.756979
2.776982	173.967221	4.761984
3.011853	171.804481	4.766989
3.125148	175.437522	4.771994
3.014109	179.159275	4.776998
3.184071	168.426782	4.782003
2.954942	167.759934	4.787008
3.182295	171.849766	4.792013
3.099794	168.622830	4.797018
3.161882	164.775451	4.802022
3.350352	171.225102	4.807027
2.840478	168.219727	4.812032
3.350917	163.967192	4.817037
3.515496	167.215771	4.822042
3.005778	163.897170	4.827046
3.344250	169.181383	4.832051
2.913793	165.436000	4.837056
3.306749	166.504057	4.842061
3.104566	168.284854	4.847066
3.405825	168.519327	4.852070
3.250618	165.249930	4.857075
3.316881	172.544324	4.862080
3.470140	174.225489	4.867085
3.381000	170.996423	4.872090
3.096671	161.407148	4.877094
3.445512	166.518908	4.882099
3.026009	173.427041	4.887104
3.529372	177.543500	4.892109
3.341660	186.585823	4.897114
3.276734	177.772278	4.902118
3.631858	174.815717	4.907123
3.257615	182.460267	4.912128
3.679183	185.434726	4.917133
3.612818	180.139401	4.922138
3.358996	177.230196	4.927142
3.382277	171.092036	4.932147
3.248124	183.552267	4.937152
3.684410	178.083773	4.942157
3.602822	177.314862	4.947162
3.506049	178.639498	4.952166
3.661338	175.404011	4.957171
3.403132	178.262850	4.962176
3.591085	169.466883	4.967181
3.297517	179.427328	4.972186
3.320449	188.553911	4.977190
3.670123	192.428555	4.982195
3.701871	189.705833	4.987200
3.629321	189.071552	4.992205
3.648968	194.484504	4.997210
3.870679	183.724963	5.002214
3.671510	184.189207	5.007219
3.471388	190.629766	5.012224
3.603437	190.387561	5.017229
3.599203	185.079398	5.022234
3.349805	185.532481	5.027238
3.652674	176.120685	5.032243
3.435394	191.814476	5.037248
3.316846	190.630551	5.042253
3.272899	191.915327	5.047258
3.587230	186.358253	5.052262
3.552697	193.019798	5.057267
3.631218	195.294716	5.062272
4.040625	203.095667	5.067277
3.659767	197.191259	5.072282
3.657643	203.088482	5.077286
3.682601	199.379750	5.082291
3.834634	210.153497	5.087296
4.127463	206.472658	5.092301
3.995825	212.187574	5.097306
3.896748	220.048719	5.102310
4.030248	200.409819	5.107315
3.841731	196.493886	5.112320
3.813877	195.153475	5.117325
4.363322	202.654219	5.122330
3.872587	189.427209	5.127334
3.836526	185.221794	5.132339
3.593209	194.291760	5.137344
3.818899	200.637553	5.142349
3.909534	213.173535	5.147354
3.947903	207.491746	5.152358
4.233442	214.533724	5.157363
4.243434	212.693887	5.162368
4.070386	204.830445	5.167373
4.021730	211.889655	5.172378
4.236411	204.266395	5.177382
4.481102	202.817112	5.182387
4.065539	197.769135	5.187392
4.099925	191.271745	5.192397
3.994655	188.168570	5.197402
4.121884	199.493488	5.202406
3.878737	208.436888	5.207411
3.843962	200.801850	5.212416
4.101029	196.237590	5.217421
4.166931	187.761165	5.222426
4.139677	203.001448	5.227430
4.119554	199.480065	5.232435
3.882891	199.311085	5.237440
4.086032	189.702844	5.242445
4.377011	210.502770	5.247450
4.120477	202.731420	5.252454
4.237200	207.006159	5.257459
3.979913	210.810797	5.262464
4.206002	203.078197	5.267469
4.048383	206.772407	5.272474
4.187707	207.405406	5.277478
4.365099	207.307997	5.282483
4.228815	212.890762	5.287488
4.668753	207.832967	5.292493
4.471801	207.717914	5.297498
4.268152	208.571987	5.302502
4.221323	204.694102	5.307507
4.318948	209.677314	5.312512
4.372024	209.070928	5.317517
4.503872	212.875090	5.322522
4.724846	215.801694	5.327526
4.863612	201.913529	5.332531
4.604798	204.484573	5.337536
4.153940	204.045231	5.342541
4.260845	205.249574	5.347546
4.247204	196.905749	5.352550
4.470447	207.719027	5.357555
4.258132	220.979208	5.362560
4.812372	230.032580	5.367565
4.963934	222.042663	5.372570
4.930164	209.184240	5.377574
4.656648	199.599589	5.382579
4.512736	201.159350	5.387584
4.333374	203.351038	5.392589
4.637340	203.961566	5.397594
4.347224	205.512455	5.402598
5.114351	205.886360	5.407603
4.526563	211.311638	5.412608
4.448000	200.421672	5.417613
4.794124	211.402477	5.422618
4.693433	214.992915	5.427622
4.612929	210.769104	5.432627
4.897548	217.940937	5.437632
4.713324	213.575091	5.442637
4.944032	211.602815	5.447642
4.511500	212.856347	5.452646
4.840533	223.956876	5.457651
4.909650	233.256620	5.462656
5.064343	220.504885	5.467661
4.722086	215.157595	5.472666
4.663258	209.785160	5.477670
4.252935	212.892310	5.482675
4.387571	231.685525	5.487680
4.532991	225.696005	5.492685
4.547850	226.547695	5.497690
4.440724	233.581217	5.502694
4.827321	225.311100	5.507699
4.833627	229.128485	5.512704
5.246750	232.290923	5.517709
4.886792	235.994497	5.522714
5.030341	234.174990	5.527718
5.019152	230.997050	5.532723
4.717065	236.994769	5.537728
4.545578	232.649081	5.542733
4.676437	231.790144	5.547738
4.932201	244.186546	5.552742
5.478268	240.241650	5.557747
5.199661	246.621686	5.562752
5.375458	246.932640	5.567757
5.350169	240.033245	5.572762
5.109237	232.547347	5.577766
5.166089	232.743946	5.582771
5.102298	231.728659	5.587776
5.224859	221.971598	5.592781
4.869777	227.063264	5.597786
5.060101	231.095601	5.602790
5.084137	226.874491	5.607795
4.746603	232.858746	5.612800
4.997107	234.996164	5.617805
5.559619	248.290748	5.622810
5.067925	250.898057	5.627814
5.379239	238.099778	5.632819
5.260693	245.049663	5.637824
5.057091	239.168262	5.642829
5.221445	232.372218	5.647834
5.167743	244.168249	5.652838
5.324301	245.466102	5.657843
5.365325	255.042308	5.662848
5.195372	253.195682	5.667853
5.551122	250.068173	5.672858
5.258076	254.479487	5.677862
5.621578	253.413489	5.682867
5.260448	256.889465	5.687872
4.996651	246.717994	5.692877
5.237648	246.661301	5.697882
5.107991	261.053894	5.702886
5.338915	244.082578	5.707891
5.226906	252.954964	5.712896
5.372187	253.672457	5.717901
5.289652	257.152511	5.722906
5.300584	256.859562	5.727910
5.759111	250.833938	5.732915
5.293672	259.843611	5.737920
5.585728	253.214334	5.742925
5.781159	259.457294	5.747930
5.677334	254.746733	5.752934
5.907219	248.639653	5.757939
5.604889	252.549387	5.762944
5.435240	243.669859	5.767949
5.147216	250.889736	5.772954
5.356273	256.659186	5.777958
5.689432	251.156107	5.782963
5.859845	252.167072	5.787968
5.541062	253.637009	5.792973
5.836756	255.156803	5.797978
5.738548	252.922529	5.802982
5.776169	247.879907	5.807987
5.397952	253.395951	5.812992
5.515527	250.612401	5.817997
5.682477	254.907805	5.823002
5.597512	254.892372	5.828006
5.844277	243.303174	5.833011
5.534648	256.885410	5.838016
5.507827	249.622426	5.843021
5.638250	258.203975	5.848026
5.666012	254.029734	5.853030
5.659906	256.109034	5.858035
5.469427	255.682933	5.863040
5.709496	254.484296	5.868045
5.405568	251.095673	5.873050
6.108231	260.869417	5.878054
5.851993	248.858669	5.883059
5.588320	260.288779	5.888064
5.566100	272.102072	5.893069
5.676020	273.704575	5.898074
6.031697	286.148723	5.903078
5.790372	272.376629	5.908083
5.476009	283.001579	5.913088
5.717652	278.654830	5.918093
6.064134	276.500010	5.923098
5.790307	280.601462	5.928102
5.899608	280.229923	5.933107
5.880891	275.610507	5.938112
5.791103	280.316041	5.943117
6.290222	282.224935	5.948122
6.168136	276.118863	5.953126
6.221455	272.886580	5.958131
6.006976	278.472049	5.963136
6.020423	279.577056	5.968141
6.370146	275.653232	5.973146
6.085105	275.618331	5.978150
6.392177	277.092065	5.983155
6.243123	286.359368	5.988160
6.181813	273.739300	5.993165
6.421754	267.871087	5.998170
6.280195	271.575465	6.003174
6.254461	272.851083	6.008179
5.819253	283.305028	6.013184
6.024512	280.605895	6.018189
5.864362	280.146598	6.023194
5.898738	288.236926	6.028198
6.051647	272.413493	6.033203
5.807172	276.080113	6.038208
5.971078	278.537896	6.043213
6.239780	278.128884	6.048218
5.952823	279.998819	6.053222
5.995582	285.461984	6.058227
5.853083	281.405992	6.063232
5.973554	291.684842	6.068237
6.273177	291.558911	6.073242
6.033947	298.875612	6.078246
6.657972	302.261485	6.083251
6.322659	294.372649	6.088256
6.352219	279.103078	6.093261
6.383152	281.439199	6.098266
5.734631	287.715496	6.103270
6.066422	277.666406	6.108275
6.295438	285.293003	6.113280
6.452733	289.191294	6.118285
6.398557	279.654704	6.123290
6.057237	285.494037	6.128294
6.257426	278.796797	6.133299
6.189989	281.856899	6.138304
6.184469	278.478756	6.143309
6.244938	280.870389	6.148314
6.030908	279.774089	6.153318
6.272059	278.768267	6.158323
5.926627	287.477701	6.163328
6.188265	275.490706	6.168333
6.370932	277.701964	6.173338
5.967053	281.624352	6.178342
6.367777	275.313498	6.183347
5.949816	280.620608	6.188352
6.173908	283.100658	6.193357
6.360712	275.538654	6.198362
6.510795	279.934763	6.203366
6.323909	271.250889	6.208371
5.911252	284.589766	6.213376
5.952302	282.757740	6.218381
6.076274	283.677864	6.223386
6.218849	290.666203	6.228390
6.415606	283.333595	6.233395
5.893211	282.857933	6.238400
5.901499	284.640772	6.243405
6.528547	294.619293	6.248410
6.473720	289.812511	6.253414
6.359980	283.936086	6.258419
6.225069	282.912887	6.263424
5.922809	288.183003	6.268429
5.933121	282.704870	6.273434
5.850883	292.872915	6.278438
6.315304	297.985700	6.283443
6.318863	302.584959	6.288448
6.182108	289.397671	6.293453
6.164255	288.833963	6.298458
6.126789	291.721725	6.303462
6.324325	286.046766	6.308467
5.984675	300.971949	6.313472
6.393396	306.944441	6.318477
6.279861	292.731664	6.323482
6.151218	289.885205	6.328486
6.347160	288.680782	6.333491
6.233747	285.793989	6.338496
6.223539	281.723728	6.343501
6.137938	288.978541	6.348506
6.361374	290.199548	6.353510
6.475422	282.262899	6.358515
6.094152	287.880667	6.363520
5.800513	285.977367	6.368525
6.455902	285.761244	6.373530
6.075002	288.496838	6.378534
6.271583	286.444448	6.383539
6.168715	282.603744	6.388544
5.929077	287.522432	6.393549
5.974348	282.820287	6.398554
5.890097	287.803364	6.403558
6.573738	300.920944	6.408563
6.484652	304.006567	6.413568
6.110481	298.426944	6.418573
6.276643	293.158656	6.423578
6.028547	294.854867	6.428582
6.227641	290.989293	6.433587
6.171974	286.578103	6.438592
5.817255	293.722962	6.443597
6.254590	289.383707	6.448602
6.092648	298.077232	6.453606
6.235379	294.470364	6.458611
6.579888	296.476096	6.463616
6.242200	286.910880	6.468621
6.059098	285.654744	6.473626
6.151149	293.862642	6.478630
6.146690	285.362325	6.483635
6.026761	285.010658	6.488640
6.122578	281.186475	6.493645
6.341574	285.290289	6.498650
5.892202	288.511096	6.503654
6.387411	297.599004	6.508659
6.265300	291.970647	6.513664
6.100230	294.068374	6.518669
6.145840	288.258885	6.523674
6.475662	294.787810	6.528678
6.258696	285.852354	6.533683
6.119207	293.558476	6.538688
6.288964	285.812464	6.543693
6.222866	285.338523	6.548698
6.144588	288.659737	6.553702
6.406098	284.642080	6.558707
6.053455	283.564198	6.563712
5.754970	287.495487	6.568717
6.357700	285.484262	6.573722
6.082310	299.352259	6.578726
6.334360	292.618466	6.583731
6.195013	288.470236	6.588736
6.113514	290.735281	6.593741
6.368315	289.423619	6.598746
6.167291	294.877287	6.603750
5.955917	297.466267	6.608755
6.159183	292.540208	6.613760
5.915438	295.817585	6.618765
6.249705	296.027938	6.623770
6.201874	310.433140	6.628774
6.669857	305.424734	6.633779
6.341756	296.392683	6.638784
5.868071	296.611775	6.643789
6.379529	296.338970	6.648794
6.021678	294.322282	6.653798
6.000084	294.600697	6.658803
5.761947	298.231533	6.663808
6.212365	315.925328	6.668813
6.434956	308.126789	6.673818
6.358407	315.914867	6.678822
6.329129	299.426928	6.683827
6.205224	294.387296	6.688832
6.228140	290.691518	6.693837
6.340199	290.588463	6.698842
6.028548	283.363486	6.703846
5.921771	289.267539	6.708851
5.996132	288.297177	6.713856
6.044896	302.314018	6.718861
6.432970	307.593713	6.723866
6.337920	310.825796	6.728870
6.435379	296.219504	6.733875
6.112869	297.000341	6.738880
5.908936	294.776196	6.743885
6.102262	284.024177	6.748890
5.830018	302.096223	6.753894
6.195040	303.137001	6.758899
6.651759	311.443151	6.763904
5.952037	296.296603	6.768909
6.414965	301.181836	6.773914
6.270599	298.075238	6.778918
6.204481	295.070350	6.783923
6.302132	292.505027	6.788928
6.055243	295.001462	6.793933
6.084850	277.925420	6.798938
5.943456	296.081489	6.803942
6.253251	304.960992	6.808947
6.511436	303.952517	6.813952
6.197094	306.177888	6.818957
6.227168	280.240282	6.823962
6.307363	292.236955	6.828966
6.090768	284.487824	6.833971
6.190990	290.277393	6.838976
6.037102	285.647384	6.843981
5.984999	282.463150	6.848986
5.981443	305.577407	6.853990
6.242066	306.760988	6.858995
6.268373	307.424242	6.864000
6.533191	306.857649	6.869005
6.338861	301.708760	6.874010
5.687867	290.006214	6.879014
6.425312	297.699186	6.884019
6.451859	287.172445	6.889024
5.803055	289.298031	6.894029
5.858318	293.746872	6.899034
6.300078	310.119588	6.904038
6.061540	311.551725	6.909043
6.442281	308.145074	6.914048
6.381826	309.239443	6.919053
6.261431	304.034750	6.924058
5.989689	292.611669	6.929062
6.209064	296.171272	6.934067
6.113959	302.940364	6.939072
6.349895	313.223394	6.944077
6.534721	292.693731	6.949082
6.229307	292.699966	6.954086
5.791674	290.866541	6.959091
6.241640	292.112387	6.964096
6.337535	302.271685	6.969101
6.226088	289.238641	6.974106
5.838370	287.403772	6.979110
6.090638	292.657152	6.984115
6.437120	297.573169	6.989120
6.250744	302.220982	6.994125
6.218163	289.770432	6.999130
6.073732	287.220655	7.004134
6.033872	280.972068	7.009139
6.008632	293.684332	7.014144
6.167314	304.447611	7.019149
6.414556	297.689255	7.024154
6.250152	298.882065	7.029158
6.380491	290.496796	7.034163
6.279652	295.235691	7.039168
5.900657	292.877454	7.044173
6.102365	292.782587	7.049178
6.309200	292.715394	7.054182
6.333483	293.141686	7.059187
5.954518	290.296238	7.064192
6.149913	297.469341	7.069197
6.445148	303.124150	7.074202
6.000617	299.017106	7.079206
6.000533	289.051318	7.084211
6.239845	305.436568	7.089216
6.035800	304.291257	7.094221
6.910976	304.736925	7.099226
6.263479	297.605360	7.104230
6.079774	291.129235	7.109235
6.013331	285.988911	7.114240
5.464156	292.157995	7.119245
6.310111	293.199821	7.124250
6.095667	310.497265	7.129254
6.342402	298.325916	7.134259
6.378374	310.506654	7.139264
6.307972	305.145483	7.144269
6.476628	297.032650	7.149274
5.965904	299.990935	7.154278
5.971076	294.295305	7.159283
5.699694	287.722103	7.164288
5.891633	300.951039	7.169293
6.072067	304.200339	7.174298
6.326757	312.107682	7.179302
6.454035	309.202392	7.184307
7.013297	311.655571	7.189312
6.383549	299.443521	7.194317
6.309092	292.766891	7.199322
6.093368	286.488738	7.204326
5.933938	290.157937	7.209331
6.093168	282.473676	7.214336
6.055010	286.532109	7.219341
6.240054	286.560056	7.224346
5.964450	296.571552	7.229350
6.101067	305.405254	7.234355
6.183539	312.418778	7.239360
6.375223	312.448855	7.244365
6.439774	308.389094	7.249370
6.115752	296.556543	7.254374
6.028292	286.749891	7.259379
6.420736	292.073193	7.264384
6.203107	296.244990	7.269389
6.135979	286.691431	7.274394
5.936708	284.567799	7.279398
6.105937	299.087890	7.284403
6.222556	302.932407	7.289408
6.322080	307.333232	7.294413
6.306683	298.429659	7.299418
5.976340	288.527947	7.304422
6.120319	295.063662	7.309427
6.405850	310.056026	7.314432
5.900592	302.725146	7.319437
6.360981	298.980235	7.324442
6.292019	309.589139	7.329446
6.172824	306.481784	7.334451
6.186797	298.823296	7.339456
5.779616	290.926669	7.344461
6.082981	294.457376	7.349466
5.858510	306.529968	7.354470
6.470486	307.665172	7.359475
5.767891	302.978224	7.364480
5.978943	308.187407	7.369485
6.517660	302.025896	7.374490
6.524525	310.297684	7.379494
6.441541	303.748926	7.384499
6.568282	307.914564	7.389504
5.829356	293.840286	7.394509
6.396000	302.948711	7.399514
6.139775	311.261461	7.404518
6.435618	307.130889	7.409523
6.185837	301.484443	7.414528
5.981284	292.145262	7.419533
6.335502	283.731467	7.424538
6.072199	292.491390	7.429542
6.338315	298.327898	7.434547
5.653043	288.127114	7.439552
5.842662	300.641419	7.444557
6.359157	306.363018	7.449562
6.397054	310.409614	7.454566
6.394606	314.598532	7.459571
6.239065	309.206325	7.464576
6.366855	310.844013	7.469581
6.263510	286.964586	7.474586
6.112967	292.568577	7.479590
5.940182	289.529679	7.484595
6.565767	294.940067	7.489600
6.245868	300.567266	7.494605
6.378374	286.774920	7.499610
6.561804	289.818111	7.504614
6.370072	288.683538	7.509619
6.024135	293.900346	7.514624
6.163902	293.008382	7.519629
6.297533	285.321778	7.524634
6.051139	279.545101	7.529638
6.023494	292.352649	7.534643
6.046151	290.033115	7.539648
5.883529	294.303913	7.544653
6.156358	286.927822	7.549658
6.261775	293.681508	7.554662
6.132045	288.294779	7.559667
6.082642	288.492104	7.564672
6.116630	293.931327	7.569677
6.429503	294.300032	7.574682
6.039814	298.976335	7.579686
5.930854	286.110582	7.584691
6.583834	296.926607	7.589696
6.325307	299.133795	7.594701
6.266069	281.296480	7.599706
5.926534	287.850527	7.604710
6.012538	284.157583	7.609715
6.329823	286.414320	7.614720
5.784708	286.603406	7.619725
6.276674	295.967058	7.624730
6.388801	298.727129	7.629734
6.626663	300.445753	7.634739
6.324889	289.103279	7.639744
6.101669	295.889151	7.644749
6.183317	281.199914	7.649754
5.990393	291.875563	7.654758
5.993129	286.123368	7.659763
5.965869	287.880105	7.664768
5.878388	308.963693	7.669773
6.429479	318.330807	7.674778
6.532178	320.238152	7.679782
5.936173	307.808875	7.684787
6.467841	297.538833	7.689792
6.515182	301.764287	7.694797
6.364255	290.784296	7.699802
6.449939	284.519324	7.704806
5.949962	293.189550	7.709811
6.489596	297.407956	7.714816
5.804738	299.017149	7.719821
6.311714	293.572414	7.724826
6.147264	295.714336	7.729830
5.853263	291.533237	7.734835
6.292715	284.460229	7.739840
5.792263	291.510721	7.744845
5.934541	288.808738	7.749850
5.998372	302.256934	7.754854
6.091588	320.129732	7.759859
6.393501	310.284588	7.764864
6.336252	309.464427	7.769869
6.369559	308.981335	7.774874
6.266285	302.097222	7.779878
6.148071	299.170046	7.784883
6.242764	283.456905	7.789888
5.792015	293.929094	7.794893
6.343868	291.701169	7.799898
6.223381	296.534870	7.804902
6.236872	301.622954	7.809907
5.783145	297.912803	7.814912
6.131168	301.888966	7.819917
6.293551	310.392799	7.824922
6.355704	314.770971	7.829926
6.474787	307.475756	7.834931
6.087190	293.612527	7.839936
6.079817	294.369607	7.844941
6.533621	298.224898	7.849946
6.371924	308.569835	7.854950
6.211989	289.258093	7.859955
6.010084	295.401581	7.864960
5.935014	293.590797	7.869965
6.496218	285.087828	7.874970
6.203001	290.264790	7.879974
6.220083	286.240898	7.884979
6.409505	291.010528	7.889984
6.078294	292.482402	7.894989
6.268930	283.897928	7.899994
6.287037	286.821328	7.904998
6.202755	279.013635	7.910003
6.422591	285.936160	7.915008
6.364432	299.362219	7.920013
6.592107	293.606637	7.925018
6.259791	293.003306	7.930022
6.140852	290.671017	7.935027
6.391755	286.873306	7.940032
6.071888	286.438876	7.945037
6.281440	286.507299	7.950042
5.966068	291.864877	7.955046
6.195020	287.409372	7.960051
6.442690	286.222205	7.965056
6.106239	290.247989	7.970061
6.298305	282.444723	7.975066
6.223379	290.200901	7.980070
5.879084	290.849091	7.985075
6.111090	287.570002	7.990080
5.930788	295.067348	7.995085
5.830019	283.386704	8.000090
6.024027	294.191932	8.005094
6.047883	289.904398	8.010099
6.167158	285.007236	8.015104
5.681796	295.940386	8.020109
5.858325	287.861915	8.025126
5.947555	298.857776	8.030144
6.336382	303.404248	8.035162
6.532404	301.887244	8.040179
6.675275	305.389635	8.045197
6.391198	291.192379	8.050214
6.043202	289.873679	8.055232
5.754223	283.985928	8.060250
6.040270	294.941676	8.065267
6.476358	304.753825	8.070285
6.763956	301.073587	8.075302
6.048909	297.947066	8.080320
5.950266	290.451870	8.085338
6.295903	282.871726	8.090355
6.222360	290.349171	8.095373
6.170501	281.167908	8.100390
6.241336	294.337692	8.105408
6.378577	293.927995	8.110426
6.367301	291.616495	8.115443
6.005306	292.868646	8.120461
6.118937	295.233255	8.125478
6.558194	299.989612	8.130496
6.540666	293.942836	8.135514
6.267182	286.550599	8.140531
6.060344	288.819944	8.145549
6.385797	304.086444	8.150566
6.767795	299.214463	8.155584
6.716749	291.399450	8.160602
6.390685	288.736199	8.165619
6.055926	286.585512	8.170637
6.043298	285.482824	8.175654
6.159122	283.034779	8.180672
6.381747	287.288408	8.185690
6.339833	287.490393	8.190707
6.141001	289.771115	8.195725
6.362727	292.402898	8.200742
6.339308	297.710946	8.205760
6.292942	301.476316	8.210778
6.718814	306.720724	8.215795
6.575957	298.976803	8.220813
6.362599	286.292703	8.225830
6.032739	286.094579	8.230848
6.356812	300.490341	8.235866
6.663396	297.084842	8.240883
6.595041	308.288270	8.245901
6.318338	292.376364	8.250918
6.148595	293.958322	8.255936
6.247714	303.340126	8.260954
6.423282	297.859696	8.265971
6.385805	305.000192	8.270989
6.566618	301.636364	8.276006
6.664013	310.406250	8.281024
6.382039	306.104678	8.286042
6.873081	305.797675	8.291059
6.498396	301.018262	8.296077
6.255085	298.452572	8.301094
6.287792	303.474188	8.306112
6.289266	306.859747	8.311130
6.462875	297.390922	8.316147
6.321110	313.746282	8.321165
6.546014	307.245214	8.326182
6.607985	307.159642	8.331200
6.187029	304.536408	8.336218
6.311669	301.335950	8.341235
6.295800	305.860232	8.346253
6.427154	305.258958	8.351270
6.748742	304.539708	8.356288
6.309270	306.466602	8.361306
6.655642	295.923213	8.366323
6.399092	304.663004	8.371341
6.612622	301.893649	8.376358
6.540684	301.459718	8.381376
6.319404	306.754396	8.386394
6.466582	308.694086	8.391411
6.368038	314.676516	8.396429
6.651814	307.099682	8.401446
6.700217	301.244598	8.406464
6.372944	311.472232	8.411482
6.535057	302.131418	8.416499
6.321131	310.668927	8.421517
6.219102	312.082562	8.426534
6.727486	314.912701	8.431552
7.083932	321.401770	8.436570
6.973957	310.714842	8.441587
6.690438	316.981677	8.446605
6.548067	307.195991	8.451622
6.940565	307.608035	8.456640
6.418344	309.645637	8.461658
6.550218	309.927855	8.466675
6.421616	306.795226	8.471693
6.574043	313.622153	8.476710
6.368292	308.371493	8.481728
6.546059	321.997991	8.486746
6.973665	315.657853	8.491763
6.872279	312.366361	8.496781
7.133625	306.487587	8.501798
7.058529	301.043028	8.506816
6.622658	313.717396	8.511834
6.769756	313.681682	8.516851
6.726735	315.455338	8.521869
6.629993	306.508255	8.526886
6.800876	305.484284	8.531904
6.773896	310.647732	8.536922
6.552300	299.908766	8.541939
6.897821	301.325298	8.546957
6.760099	313.224298	8.551974
6.982297	306.581649	8.556992
6.552505	305.600712	8.562010
6.787588	298.400670	8.567027
6.830321	300.467068	8.572045
6.913620	300.674803	8.577063
6.756179	301.585855	8.582080
6.427702	306.098852	8.587098
6.866482	306.257551	8.592115
6.955369	302.554606	8.597133
6.620918	305.768418	8.602151
6.594320	297.776037	8.607168
6.467270	302.434386	8.612186
6.682968	304.088869	8.617203
6.757555	306.551071	8.622221
6.606735	307.893412	8.627239
6.857946	315.020521	8.632256
6.961263	326.904091	8.637274
7.082920	312.577378	8.642291
6.725003	310.584919	8.647309
6.335297	305.930912	8.652327
6.711225	310.208012	8.657344
6.865199	325.267713	8.662362
7.040277	319.484412	8.667379
7.198145	320.772382	8.672397
7.054591	322.328176	8.677415
6.934400	307.284929	8.682432
6.835143	309.351346	8.687450
6.884483	295.638629	8.692467
6.883226	306.623339	8.697485
6.784969	317.159281	8.702503
6.892233	315.592982	8.707520
7.124589	328.377903	8.712538
6.946155	325.117338	8.717555
6.848761	317.902786	8.722573
6.986106	321.986675	8.727591
6.887579	317.464044	8.732608
6.972212	323.765075	8.737626
6.925606	321.171911	8.742643
7.035922	321.406995	8.747661
6.904627	322.162508	8.752679
6.959202	324.690941	8.757696
7.064663	336.132396	8.762714
6.955674	315.353632	8.767731
7.297130	316.780265	8.772749
6.412786	316.551714	8.777767
6.838292	322.957452	8.782784
6.811723	325.804614	8.787802
7.265754	324.095967	8.792819
7.106676	325.928717	8.797837
7.331741	329.790679	8.802855
7.311401	317.827542	8.807872
7.184223	309.068222	8.812890
6.938290	305.546787	8.817907
7.130550	301.086177	8.822925
6.764360	302.178045	8.827943
7.049426	312.322963	8.832960
7.018496	327.736483	8.837978
6.958947	326.028907	8.842995
7.120605	326.360134	8.848013
7.044814	333.203667	8.853031
6.944430	325.771840	8.858048
6.872907	335.404279	8.863066
7.038746	325.450682	8.868083
7.016169	331.209862	8.873101
6.938430	321.865359	8.878119
7.104167	319.807146	8.883136
7.389148	323.072833	8.888154
7.138147	318.788524	8.893171
7.349363	322.785176	8.898189
7.012886	331.972900	8.903207
7.202237	325.638297	8.908224
6.994720	324.774222	8.913242
6.968490	316.257942	8.918259
7.399542	327.172199	8.923277
7.468381	324.892400	8.928295
7.397254	323.047780	8.933312
7.420934	324.971989	8.938330
7.489493	324.957970	8.943347
7.138904	307.239917	8.948365
6.882263	311.031716	8.953383
7.108624	318.500347	8.958400
7.250627	325.234232	8.963418
7.200268	325.232417	8.968435
7.344167	322.833641	8.973453
7.387913	326.080086	8.978471
7.469870	320.639469	8.983488
7.359258	326.181994	8.988506
7.110433	310.710674	8.993523
7.267972	316.075754	8.998541
7.114215	327.137865	9.003559
7.255039	323.837060	9.008576
7.316792	322.694388	9.013594
7.202139	329.695440	9.018611
7.471256	326.226346	9.023629
6.925198	329.564622	9.028647
7.363186	325.968255	9.033664
6.976659	336.747895	9.038682
7.294310	331.084397	9.043699
7.572114	323.489552	9.048717
7.277156	335.750700	9.053735
7.391911	331.595622	9.058752
7.425058	317.361577	9.063770
7.354172	331.276091	9.068787
7.653745	322.453477	9.073805
7.386939	325.420089	9.078823
7.536043	322.439868	9.083840
7.243727	327.281736	9.088858
7.342593	336.527905	9.093875
7.600974	328.033575	9.098893
7.035694	330.286155	9.103911
7.096275	326.357251	9.108928
7.274437	325.306902	9.113946
7.263464	324.311245	9.118963
7.383617	325.601931	9.123981
7.318828	337.577950	9.128999
7.079163	324.512932	9.134016
7.306372	318.958187	9.139034
7.398777	331.297868	9.144051
7.619010	320.894018	9.149069
7.370429	333.138476	9.154087
6.922676	330.257494	9.159104
7.296965	329.053538	9.164122
6.875177	330.441226	9.169139
7.348407	337.129856	9.174157
7.305710	344.454207	9.179175
7.665121	341.384438	9.184192
7.572536	345.062344	9.189210
7.696155	345.402649	9.194227
7.736751	341.486321	9.199245
7.202497	337.028371	9.204263
7.388175	339.962403	9.209280
7.428961	343.786791	9.214298
7.431266	348.500747	9.219315
7.762869	344.636934	9.224333
7.559721	346.571216	9.229351
7.673227	346.411351	9.234368
7.689647	348.324070	9.239386
8.077491	338.604129	9.244403
7.735394	338.729783	9.249421
7.520263	328.945947	9.254439
7.415943	329.599436	9.259456
7.473492	320.622011	9.264474
7.099575	330.541356	9.269491
7.681458	333.606192	9.274509
7.659647	351.937265	9.279527
7.862647	346.297923	9.284544
7.975424	336.699701	9.289562
7.458149	333.539225	9.294579
7.457576	324.779119	9.299597
7.710975	336.077627	9.304615
7.748597	338.750704	9.309632
7.890338	333.404911	9.314650
7.160749	328.794349	9.319667
7.865344	334.733786	9.324685
7.585142	353.165047	9.329703
7.750730	344.142389	9.334720
7.945924	350.483016	9.339738
7.521412	334.878092	9.344755
7.809484	336.448730	9.349773
7.559429	342.666185	9.354791
7.587098	344.091186	9.359808
7.594188	348.851731	9.364826
7.755189	353.916499	9.369843
8.131764	351.137529	9.374861
7.703686	354.416418	9.379879
7.908544	351.686273	9.384896
7.625732	342.430490	9.389914
7.565815	342.953996	9.394931
7.734236	346.215746	9.399949
7.668222	350.170366	9.404967
7.679574	340.638423	9.409984
7.643901	343.742611	9.415002
7.937697	346.473629	9.420019
7.776800	348.098393	9.425037
7.972634	349.525613	9.430055
7.891630	348.632371	9.435072
7.994158	347.136231	9.440090
7.677544	348.860974	9.445107
7.672443	347.447860	9.450125
7.885914	352.277253	9.455143
7.980299	341.211370	9.460160
8.064736	335.940765	9.465178
7.756207	341.794961	9.470195
7.861062	342.696733	9.475213
7.776779	343.874092	9.480231
7.838219	352.116297	9.485248
7.898478	347.550002	9.490266
7.959417	350.812709	9.495283
7.599042	348.176881	9.500301
7.058931	360.987426	9.505319
7.691166	344.334386	9.510336
7.901175	346.687152	9.515354
7.556782	348.839074	9.520371
7.579111	348.977412	9.525389
7.793301	347.239837	9.530407
8.034445	365.315400	9.535424
8.415447	360.093283	9.540442
7.997551	354.118289	9.545459
7.843293	358.916581	9.550477
7.697755	347.345281	9.555495
8.004235	354.836164	9.560512
8.150140	349.281446	9.565530
7.847491	352.992060	9.570547
8.019992	345.527204	9.575565
8.188420	354.330232	9.580583
7.601804	345.617182	9.585600
7.969940	359.501231	9.590618
7.956578	370.762404	9.595635
8.334199	367.175428	9.600653
8.422148	365.135632	9.605671
8.094888	352.680646	9.610688
7.853353	346.343699	9.615706
7.862744	359.750304	9.620723
7.893241	355.305399	9.625741
8.260657	374.263821	9.630759
8.168387	372.182660	9.635776
8.168734	366.710556	9.640794
7.702547	370.777977	9.645811
8.222105	377.339495	9.650829
8.111751	382.793640	9.655847
8.035181	381.151822	9.660864
8.465774	378.673689	9.665882
8.012813	373.808619	9.670899
8.223549	374.921113	9.675917
8.569802	373.383868	9.680935
8.003770	360.893472	9.685952
8.244208	351.534126	9.690970
7.729383	359.285422	9.695987
8.429688	361.628121	9.701005
8.475727	368.408520	9.706023
8.441373	360.754970	9.711040
8.148113	359.361475	9.716058
7.968272	357.631602	9.721075
8.091694	352.168741	9.726093
8.255334	355.377591	9.731111
8.046427	363.488334	9.736128
8.187720	353.267159	9.741146
8.333719	369.962754	9.746163
8.767946	364.277938	9.751181
8.372157	357.677843	9.756199
7.927050	358.687332	9.761216
8.073094	351.999721	9.766234
8.458643	371.018428	9.771251
8.283575	359.101444	9.776269
8.278911	362.797221	9.781287
7.891539	358.168082	9.786304
8.540570	357.931149	9.791322
8.094646	369.546832	9.796339
8.341686	365.576267	9.801357
8.618865	371.626441	9.806375
8.143180	372.463977	9.811392
8.417530	365.797407	9.816410
8.457605	370.615935	9.821427
8.410467	373.999609	9.826445
8.302845	367.578693	9.831463
8.565019	373.085281	9.836480
8.246162	356.643423	9.841498
8.385500	373.838648	9.846515
8.406151	373.699551	9.851533
8.370975	370.255736	9.856551
8.373155	380.135486	9.861568
8.550358	370.107515	9.866586
8.497246	377.319898	9.871603
8.074893	359.956930	9.876621
8.458699	368.145796	9.881639
8.363942	373.389238	9.886656
8.729559	373.723421	9.891674
8.756199	381.693363	9.896691
8.308227	356.593625	9.901709
8.444740	360.422046	9.906727
8.567978	372.422459	9.911744
8.294588	364.623098	9.916762
8.324482	363.305513	9.921779
8.681337	370.908474	9.926797
8.316018	367.045872	9.931815
8.512322	368.816984	9.936832
8.754701	372.458521	9.941850
8.474065	370.387754	9.946867
8.480920	369.635458	9.951885
8.913875	372.906516	9.956903
8.279302	363.945317	9.961920
8.769435	368.034246	9.966938
8.637285	371.137681	9.971955
8.463469	374.664148	9.976973
8.447458	368.361505	9.981991
8.564950	370.914860	9.987008
8.629548	369.850633	9.992026
8.543228	369.971175	9.997043
8.634762	371.020182	10.002061
8.932546	367.275232	10.007079
8.861742	367.134597	10.012096
8.559411	368.068211	10.017114
8.216314	366.985415	10.022131
8.473196	371.962681	10.027149
8.512757	371.826951	10.032167
8.763862	373.400193	10.037184
8.901334	371.466289	10.042202
8.790186	381.499376	10.047219
8.687532	378.602522	10.052237
8.739862	373.655624	10.057255
9.011183	376.254454	10.062272
8.903172	366.763170	10.067290
8.555401	358.574628	10.072307
8.360464	363.530725	10.077325
8.589802	365.261980	10.082343
8.432493	371.673277	10.087360
9.089039	367.093028	10.092378
8.680255	376.225765	10.097395
8.312610	375.089988	10.102413
8.826991	371.497496	10.107431
8.490998	373.086412	10.112448
8.519167	362.611461	10.117466
8.852301	371.287873	10.122483
8.248364	367.509758	10.127501
8.503359	367.286840	10.132519
8.667731	369.245950	10.137536
8.642322	373.617108	10.142554
8.719300	372.153344	10.147571
8.703177	384.450003	10.152589
8.965984	388.905671	10.157607
8.642466	396.526217	10.162624
8.817323	407.859089	10.167642
9.120710	394.617955	10.172659
9.082847	392.698725	10.177677
9.005259	399.075529	10.182695
8.929679	383.485658	10.187712
8.730882	379.707575	10.192730
9.189809	374.842530	10.197747
8.741436	374.044353	10.202765
8.873299	383.115005	10.207783
8.978649	383.669583	10.212800
8.876889	383.899820	10.217818
9.077507	388.582910	10.222835
8.985403	386.810974	10.227853
9.043346	383.885959	10.232871
9.003414	378.413812	10.237888
8.755149	377.414074	10.242906
8.722382	378.125848	10.247923
8.942576	393.658108	10.252941
9.223390	384.964609	10.257959
9.405764	398.571515	10.262976
9.329165	385.660935	10.267994
8.955839	379.432854	10.273011
8.779403	376.661091	10.278029
8.690046	371.957148	10.283047
9.103922	382.403925	10.288064
8.913710	393.080454	10.293082
9.149152	399.272829	10.298099
8.727389	401.026572	10.303117
9.119085	388.737317	10.308135
9.182097	393.410276	10.313152
9.190747	391.632119	10.318170
9.427990	386.315619	10.323187
9.090237	391.423340	10.328205
9.262076	387.423455	10.333223
9.075883	387.925601	10.338240
8.946632	390.785605	10.343258
9.164099	383.140172	10.348275
9.087558	389.557834	10.353293
9.515583	387.307305	10.358311
9.582418	383.052385	10.363328
9.167465	372.040540	10.368346
9.150213	370.995368	10.373363
8.588083	363.304076	10.378381
8.863913	373.551447	10.383399
8.859474	378.506289	10.388416
9.237754	390.056772	10.393434
9.466870	385.823919	10.398451
9.282841	393.962359	10.403469
9.386738	388.022871	10.408487
9.134426	398.320930	10.413504
8.955150	390.330189	10.418522
9.534186	386.923276	10.423539
9.350345	387.847910	10.428557
9.205385	390.287505	10.433575
9.191799	393.022210	10.438592
9.124380	393.165055	10.443610
9.162538	400.748224	10.448627
9.142108	394.307411	10.453645
9.355545	385.532888	10.458663
9.313187	391.964162	10.463680
9.515851	397.685139	10.468698
9.773138	385.404191	10.473715
9.447185	392.337186	10.478733
9.466118	391.147531	10.483751
9.345942	391.030361	10.488768
9.487476	377.767105	10.493786
9.284157	380.253653	10.498803
9.100863	392.263937	10.503821
9.067025	387.425120	10.508839
9.365449	391.162071	10.513856
9.260714	402.043037	10.518874
9.297522	390.105666	10.523891
9.171384	395.713742	10.528909
9.100990	394.111985	10.533927
9.550558	388.948608	10.538944
9.280172	390.735582	10.543962
9.097676	389.612001	10.548979
9.569927	399.768848	10.553997
9.398123	402.689126	10.559015
9.711774	414.221286	10.564032
9.583718	405.717662	10.569050
9.480664	392.722837	10.574067
9.271937	403.247630	10.579085
9.762409	400.040687	10.584103
9.905925	406.105373	10.589120
9.499450	397.793415	10.594138
9.414281	403.732769	10.599155
9.178541	396.271496	10.604173
9.703495	400.812578	10.609191
9.864512	403.927176	10.614208
9.748931	405.731072	10.619226
9.710629	397.424905	10.624243
9.117908	395.140808	10.629261
9.444304	406.611022	10.634279
9.651552	404.233929	10.639296
9.635600	417.256379	10.644314
9.614341	418.455486	10.649331
9.798236	419.619497	10.654349
9.994239	416.868631	10.659367
9.597064	409.400931	10.664384
9.504141	403.069227	10.669402
9.858415	404.727389	10.674419
9.655697	415.200763	10.679437
9.923707	412.028454	10.684455
9.770564	398.782662	10.689472
9.334399	405.404635	10.694490
9.808171	401.193644	10.699507
9.652446	414.906850	10.704525
9.721337	416.155034	10.709543
10.136066	417.636536	10.714560
9.480515	412.370675	10.719578
9.692258	408.695914	10.724595
9.929974	411.195845	10.729613
9.749428	420.274134	10.734631
10.172434	407.550825	10.739648
9.409668	393.203967	10.744666
9.525131	405.372860	10.749683
9.762551	415.730372	10.754701
9.481174	420.267621	10.759719
9.943725	414.994923	10.764736
9.792507	422.257312	10.769754
9.785317	421.601869	10.774771
9.509545	416.851203	10.779789
9.852548	421.392218	10.784807
9.788611	417.561573	10.789824
9.582895	423.986736	10.794842
10.001162	411.125314	10.799859
9.497540	417.612636	10.804877
9.555671	411.320523	10.809895
9.927585	409.965462	10.814912
9.481382	413.799419	10.819930
10.249699	424.370907	10.824947
10.182048	427.751474	10.829965
10.134859	412.860865	10.834983
10.006001	417.926602	10.840000
9.647509	424.549112	10.845018
10.003136	410.466745	10.850035
9.842209	422.404143	10.855053
9.851801	424.725010	10.860071
10.327079	421.138597	10.865088
10.025954	423.286947	10.870106
9.856007	422.918763	10.875123
10.003084	431.905025	10.880141
10.312425	432.188015	10.885159
9.809936	427.005610	10.890176
9.863281	432.850828	10.895194
10.189781	432.790337	10.900211
9.901669	440.326498	10.905229
10.348648	445.472992	10.910247
10.376492	442.060374	10.915264
10.027278	424.998363	10.920282
10.066776	413.234117	10.925299
10.064598	422.215212	10.930317
10.065882	430.040808	10.935335
10.238274	433.910994	10.940352
10.159349	430.994659	10.945370
10.466324	434.301121	10.950387
10.136853	414.291834	10.955405
9.891297	412.572187	10.960423
10.136722	426.364947	10.965440
10.093636	435.320862	10.970458
10.252762	434.740505	10.975475
10.153695	440.909240	10.980493
9.921087	436.158160	10.985511
10.429585	436.646815	10.990528
10.127046	443.973795	10.995546
10.513863	439.312455	11.000563
10.558388	437.367769	11.005581
10.217131	438.793417	11.010599
10.807717	436.227253	11.015616
10.498659	430.948462	11.020634
10.439955	418.360103	11.025651
10.277802	418.643923	11.030669
10.013964	417.589806	11.035687
10.017678	412.221300	11.040704
10.376300	420.357310	11.045722
10.515051	427.618732	11.050739
10.307680	434.788888	11.055757
9.980237	431.024511	11.060775
10.682832	427.737202	11.065792
10.414833	445.260990	11.070810
10.323790	436.877814	11.075827
10.286215	439.938136	11.080845
10.042426	437.249430	11.085863
10.272375	434.130377	11.090880
10.323012	434.920681	11.095898
10.607381	440.275519	11.100915
10.392361	437.314104	11.105933
10.422768	435.400018	11.110951
10.472970	433.000038	11.115968
10.208510	441.308804	11.120986
10.308498	429.724468	11.126003
10.305943	430.270602	11.131021
10.162402	433.076037	11.136039
10.641307	434.844178	11.141056
10.528633	428.909995	11.146074
10.253581	430.836547	11.151091
10.428783	431.651636	11.156109
10.580033	441.053797	11.161127
10.705474	434.763819	11.166144
10.530738	433.288750	11.171162
10.642035	419.815587	11.176179
10.777244	416.638709	11.181197
10.470989	434.389338	11.186215
10.583674	428.823989	11.191232
10.423934	431.972754	11.196250
10.413474	431.447202	11.201267
10.636537	436.546510	11.206285
10.322794	438.715761	11.211303
10.809897	427.935799	11.216320
10.811117	439.734360	11.221338
10.817043	433.362010	11.226355
10.929530	433.962812	11.231373
10.392980	441.768016	11.236391
10.591694	435.731703	11.241408
10.462358	433.205049	11.246426
10.588218	439.111558	11.251443
11.096421	443.614235	11.256461
10.790402	439.095479	11.261479
10.787831	430.269363	11.266496
10.681342	442.094162	11.271514
10.753649	436.083841	11.276531
10.813611	438.737677	11.281549
10.797710	440.974158	11.286567
10.896930	432.211084	11.291584
10.621711	446.223771	11.296602
10.545629	444.670229	11.301619
10.726981	442.161469	11.306637
10.543105	454.692567	11.311655
11.100496	450.995538	11.316672
10.795685	456.666164	11.321690
10.772045	455.577803	11.326707
11.118357	445.599196	11.331725
10.661378	454.524892	11.336743
11.162607	449.470213	11.341760
10.746569	459.424589	11.346778
11.288219	456.651457	11.351795
11.247030	449.418634	11.356813
10.873141	449.650219	11.361831
11.023222	441.945829	11.366848
10.957304	446.989152	11.371866
10.944529	442.118641	11.376883
11.221479	438.809243	11.381901
10.975417	437.029715	11.386919
11.101048	432.923411	11.391936
11.008132	433.414190	11.396954
10.454597	434.803464	11.401971
10.754711	440.080115	11.406989
10.844347	450.482746	11.412007
11.222277	445.008632	11.417024
10.989500	450.421901	11.422042
10.832314	447.394678	11.427059
11.008442	451.273753	11.432077
11.067564	455.821109	11.437095
11.366488	448.522709	11.442112
10.996195	455.023998	11.447130
11.285331	455.761392	11.452147
11.092823	459.486435	11.457165
11.150901	455.223395	11.462183
11.014103	454.584975	11.467200
11.139684	457.843948	11.472218
11.181135	453.075438	11.477235
11.358163	449.813152	11.482253
11.320202	454.287265	11.487271
11.143460	446.778917	11.492288
10.970935	452.848647	11.497306
10.591210	451.717902	11.502323
11.070696	452.113250	11.507341
10.787975	459.973611	11.512359
11.094032	457.641083	11.517376
11.087153	456.149345	11.522394
11.108157	452.955529	11.527411
11.190365	457.060657	11.532429
11.236842	473.648774	11.537447
11.485954	463.619022	11.542464
11.488376	469.383822	11.547482
10.899470	459.241564	11.552499
11.392514	463.721362	11.557517
11.486023	465.524266	11.562535
11.276456	469.390816	11.567552
11.264488	470.386519	11.572570
11.449853	469.682161	11.577587
11.514076	468.728434	11.582605
11.343697	473.923723	11.587623
11.126896	470.249403	11.592640
11.422988	475.880124	11.597658
11.415995	471.838639	11.602675
11.554465	470.475741	11.607693
11.485919	467.740811	11.612711
11.431905	470.986726	11.617728
11.317894	464.519434	11.622746
11.238169	473.670411	11.627763
11.527818	469.964574	11.632781
11.398229	467.728274	11.637799
11.311399	466.943226	11.642816
11.629066	477.291435	11.647834
10.970896	476.611120	11.652851
11.122368	468.903346	11.657869
11.125345	478.470617	11.662887
11.425478	473.668137	11.667904
11.603820	472.693487	11.672922
11.555672	481.303091	11.677939
11.515802	480.406594	11.682957
11.826022	476.157937	11.687975
11.717844	476.827810	11.692992
11.795616	475.060972	11.698010
11.250437	474.691252	11.703027
11.208323	472.299328	11.708045
11.264867	479.011865	11.713063
11.513057	497.323140	11.718080
11.418772	495.636734	11.723098
11.596566	494.690569	11.728115
11.974042	493.972077	11.733133
12.050565	496.841084	11.738151
12.238624	488.613233	11.743168
12.195440	479.386338	11.748186
11.766171	477.546973	11.753203
11.956451	466.800580	11.758221
11.614149	473.729841	11.763239
11.844208	465.053671	11.768256
11.579726	473.614908	11.773274
11.830617	466.011570	11.778291
12.013876	465.673595	11.783309
12.119560	461.078110	11.788327
11.812565	465.344817	11.793344
11.848886	461.646867	11.798362
11.526314	470.355995	11.803379
11.831570	458.301046	11.808397
11.895384	462.440595	11.813415
11.436783	464.136966	11.818432
11.228850	462.597640	11.823450
11.545044	486.360738	11.828467
11.996008	492.734174	11.833485
11.949270	487.196784	11.838503
12.153022	496.303636	11.843520
11.912082	486.416439	11.848538
11.893487	496.176417	11.853555
12.303259	487.068333	11.858573
12.145726	486.442608	11.863591
11.771285	484.995473	11.868608
11.951240	473.316611	11.873626
11.862766	490.563197	11.878643
12.006433	484.365032	11.883661
12.250600	489.782946	11.888679
12.087408	490.644413	11.893696
11.895730	499.333175	11.898714
11.890790	500.801133	11.903731
12.326378	489.208686	11.908749
12.243828	489.480113	11.913767
11.943606	483.404707	11.918784
12.311287	486.894222	11.923802
11.809314	489.856452	11.928819
11.859809	483.237315	11.933837
11.919385	489.015312	11.938855
11.912339	490.849653	11.943872
12.075312	482.578376	11.948890
11.961717	485.748368	11.953907
11.989416	483.695849	11.958925
12.247139	490.421247	11.963943
11.695406	487.771012	11.968960
12.111263	496.620790	11.973978
12.067488	493.705283	11.978995
12.284277	489.774112	11.984013
12.520311	490.090607	11.989031
12.222096	494.103502	11.994048
12.227245	491.634792	11.999066
12.054006	492.292706	12.004083
12.089510	489.585752	12.009101
12.440687	479.713660	12.014119
12.218141	484.961253	12.019136
12.241731	486.639353	12.024154
11.899381	493.663298	12.029171
12.550737	496.285023	12.034189
12.646655	500.750926	12.039207
12.306271	500.207315	12.044224
11.932735	484.556454	12.049242
12.341262	499.734453	12.054259
12.351375	502.295079	12.059277
12.458619	507.399817	12.064295
12.712416	509.799433	12.069312
12.714234	506.513926	12.074330
12.444093	503.955539	12.079347
12.220634	487.523952	12.084365
12.127257	494.704784	12.089383
11.885071	502.905974	12.094400
12.383575	505.232778	12.099418
12.183576	504.490593	12.104435
12.669711	510.830158	12.109453
12.778505	514.757599	12.114471
12.316779	517.142394	12.119488
12.593282	507.464941	12.124506
12.565049	510.646892	12.129523
12.523179	513.963503	12.134541
12.631786	505.230488	12.139559
12.587695	510.425059	12.144576
13.016379	507.729466	12.149594
12.856117	518.328827	12.154611
12.890583	515.991243	12.159629
12.672492	507.413229	12.164647
12.548751	514.207496	12.169664
12.494812	513.455192	12.174682
12.460336	513.949497	12.179699
12.837310	518.728234	12.184717
12.631392	509.308920	12.189735
12.567899	518.476326	12.194752
12.726736	510.786322	12.199770
13.040652	511.330520	12.204787
12.664380	514.825423	12.209805
13.019450	506.997575	12.214823
12.820883	521.553781	12.219840
12.801832	512.569252	12.224858
12.571151	511.008218	12.229875
12.721011	510.157915	12.234893
12.824743	507.970485	12.239911
12.400902	512.580429	12.244928
12.813484	511.316854	12.249946
12.728059	516.483149	12.254963
12.687134	508.294098	12.259981
12.777388	505.496570	12.264999
13.026907	508.546917	12.270016
12.613423	506.118139	12.275034
12.872206	509.230157	12.280051
12.869659	508.690747	12.285069
13.182785	509.320271	12.290087
12.810552	512.855569	12.295104
12.893797	509.333331	12.300122
12.698945	508.767062	12.305139
12.762423	511.227866	12.310157
13.097383	509.859618	12.315175
12.882617	521.341583	12.320192
13.214331	505.950110	12.325210
13.219503	502.582034	12.330227
12.742049	514.196409	12.335245
12.923709	513.426357	12.340263
12.785858	510.831594	12.345280
12.800432	503.615312	12.350298
12.918519	519.302428	12.355315
13.032549	527.716399	12.360333
13.097675	534.790522	12.365351
13.338226	539.962873	12.370368
13.193006	531.805827	12.375386
13.236306	533.809051	12.380403
13.283556	530.690026	12.385421
12.849209	521.050663	12.390439
13.202835	533.207809	12.395456
13.268900	531.777288	12.400474
13.277114	538.778226	12.405491
13.232754	537.459567	12.410509
13.498494	525.164584	12.415527
12.895557	526.403773	12.420544
13.230264	522.122892	12.425562
13.293533	528.421010	12.430579
13.147230	532.684804	12.435597
13.544425	524.162456	12.440615
13.153679	532.882228	12.445632
13.401578	522.505510	12.450650
13.659290	535.242453	12.455667
13.132304	521.979038	12.460685
13.256466	524.875344	12.465703
13.052239	526.819281	12.470720
13.435304	513.007102	12.475738
13.342682	529.146736	12.480755
13.240529	525.883724	12.485773
13.628294	528.101546	12.490791
13.466849	531.237972	12.495808
13.556501	526.225263	12.500826
13.513849	529.611424	12.505843
13.406699	527.153882	12.510861
13.524445	524.077529	12.515879
13.422492	532.168541	12.520896
13.202957	529.469733	12.525914
13.554203	530.146969	12.530931
13.603604	523.581633	12.535949
13.618126	525.873346	12.540967
13.427565	537.237949	12.545984
13.532478	536.962662	12.551002
13.741362	535.595107	12.556019
13.368534	533.693302	12.561037
13.418931	533.256097	12.566055
13.268260	535.358946	12.571072
13.348045	529.139155	12.576090
13.347307	532.461989	12.581107
13.534950	540.668854	12.586125
13.785371	526.959364	12.591143
13.218709	538.130073	12.596160
13.480688	531.219226	12.601178
13.383877	533.941665	12.606195
13.470613	542.669147	12.611213
13.661773	552.175602	12.616231
13.853284	560.340850	12.621248
13.437135	558.108131	12.626266
14.085920	555.412975	12.631283
13.743329	563.339504	12.636301
14.051733	555.039240	12.641319
13.820560	561.938610	12.646336
13.676912	558.754633	12.651354
14.013817	559.055423	12.656371
13.481313	558.749997	12.661389
13.781479	551.965734	12.666407
13.382707	558.361047	12.671424
13.650204	548.748087	12.676442
13.986220	543.346737	12.681459
13.837939	559.258390	12.686477
14.087532	553.403455	12.691495
13.571550	561.082438	12.696512
13.675018	559.851209	12.701530
13.718121	565.025908	12.706547
13.518593	566.117088	12.711565
13.800086	554.157288	12.716583
14.103402	556.675428	12.721600
13.878925	552.532092	12.726618
13.820022	557.646935	12.731635
14.051805	569.889346	12.736653
14.448856	574.478788	12.741671
13.773845	570.490798	12.746688
13.790379	564.271376	12.751706
14.095632	572.743954	12.756723
14.147299	575.537952	12.761741
14.405576	575.178828	12.766759
14.201111	560.287337	12.771776
14.090931	562.393351	12.776794
14.056657	553.723583	12.781811
14.060774	562.078947	12.786829
13.821464	567.515358	12.791847
14.065813	571.080894	12.796864
14.468966	576.928497	12.801882
14.505698	570.059017	12.806899
14.063910	584.271307	12.811917
14.433992	576.983866	12.816935
14.282613	573.662240	12.821952
13.943608	559.457543	12.826970
14.692554	574.405887	12.831987
14.386146	568.088428	12.837005
14.229017	555.751971	12.842023
14.090352	555.423093	12.847040
14.181720	574.333194	12.852058
14.640737	568.246840	12.857075
14.287211	567.484377	12.862093
14.219939	565.831627	12.867111
14.329403	573.548929	12.872128
14.227780	578.414820	12.877146
14.517158	574.620645	12.882163
14.651846	582.535986	12.887181
14.851550	569.402380	12.892199
14.225327	555.447523	12.897216
14.344763	561.386629	12.902234
14.607178	542.922831	12.907251
13.997235	552.610817	12.912269
14.486887	555.346086	12.917287
14.335952	567.376695	12.922304
14.023302	584.866549	12.927322
14.415653	567.231370	12.932339
14.098786	571.575375	12.937357
14.479773	571.967128	12.942375
14.581747	573.724546	12.947392
14.648817	580.542776	12.952410
14.749669	574.073547	12.957427
14.398432	573.859813	12.962445
14.687040	574.811879	12.967463
14.545600	576.184337	12.972480
14.471169	570.259930	12.977498
14.965943	575.572583	12.982515
15.050221	579.387095	12.987533
14.698962	573.660416	12.992551
14.827933	575.274782	12.997568
14.460488	574.142116	13.002586
14.730118	568.814208	13.007603
14.688634	576.274159	13.012621
14.461577	579.638550	13.017639
14.747382	568.460675	13.022656
14.564158	574.551045	13.027674
14.426331	565.278883	13.032691
14.630453	586.901091	13.037709
14.752767	597.342900	13.042727
15.068149	593.254351	13.047744
15.053705	605.610858	13.052762
15.668492	582.667906	13.057779
14.901359	577.005976	13.062797
14.852655	575.826840	13.067815
14.862031	573.452130	13.072832
14.856180	575.459856	13.077850
14.917406	566.614272	13.082867
14.478442	579.450250	13.087885
14.640597	579.443748	13.092903
15.057581	600.158711	13.097920
14.929950	608.531454	13.102938
14.967617	598.509302	13.107955
15.127556	603.362877	13.112973
15.168390	600.683478	13.117991
15.182477	597.648497	13.123008
14.933613	609.795363	13.128026
15.128994	590.991673	13.133043
14.964782	601.582232	13.138061
15.286014	600.111977	13.143079
15.361590	599.961172	13.148096
14.945140	589.350194	13.153114
15.344522	584.153552	13.158131
15.069120	584.413983	13.163149
15.218115	585.514013	13.168167
15.213556	577.887288	13.173184
15.455689	593.365817	13.178202
15.243500	572.763758	13.183219
15.259533	568.399944	13.188237
14.909312	571.067173	13.193255
15.487401	573.226967	13.198272
14.688147	578.813677	13.203290
15.380931	583.435968	13.208307
15.211246	594.286140	13.213325
15.517282	589.659427	13.218343
15.106111	590.499550	13.223360
15.091019	597.100215	13.228378
15.151140	591.959547	13.233395
14.973336	585.713574	13.238413
15.230521	592.458028	13.243431
15.284836	585.039874	13.248448
14.876272	594.343094	13.253466
15.285731	586.942225	13.258483
14.924733	594.496110	13.263501
15.247163	605.799820	13.268519
15.216068	615.773240	13.273536
15.322037	616.807391	13.278554
15.369345	615.496544	13.283571
15.231742	625.436061	13.288589
15.387319	617.004935	13.293607
15.353447	615.864510	13.298624
15.239022	623.253790	13.303642
15.414420	617.063262	13.308659
15.324158	612.028050	13.313677
15.500911	627.273801	13.318695
16.111288	632.174012	13.323712
15.900696	629.959771	13.328730
15.747320	623.577442	13.333747
15.631966	617.653080	13.338765
15.490466	621.281857	13.343783
15.803586	618.086710	13.348800
15.560454	628.172042	13.353818
15.573862	619.015154	13.358835
15.714637	619.674673	13.363853
15.371900	631.091431	13.368871
15.833520	635.831775	13.373888
15.937349	642.429719	13.378906
15.789276	643.604407	13.383923
16.219343	630.251860	13.388941
15.761379	632.146954	13.393959
15.822806	626.958738	13.398976
15.434244	627.239944	13.403994
15.971140	637.639318	13.409011
16.240080	642.671584	13.414029
15.940682	644.336873	13.419047
15.519639	632.224482	13.424064
15.951429	635.511549	13.429082
15.917921	641.976248	13.434099
15.970999	641.519688	13.439117
16.258549	635.188621	13.444135
16.182897	634.695302	13.449152
16.034765	631.073371	13.454170
16.022239	621.216805	13.459187
15.936084	619.077861	13.464205
15.728581	617.951847	13.469223
15.938373	626.313087	13.474240
15.972142	643.960493	13.479258
16.282001	637.673286	13.484275
16.358025	638.765748	13.489293
15.707100	647.279942	13.494311
16.258757	639.484541	13.499328
16.027494	640.145183	13.504346
16.339517	642.138137	13.509363
16.222166	629.950062	13.514381
15.954137	639.610105	13.519399
15.948759	628.493307	13.524416
15.978465	639.520736	13.529434
16.134338	634.346215	13.534451
16.136923	635.295482	13.539469
16.199927	631.015854	13.544487
16.455395	634.999376	13.549504
16.348510	644.189382	13.554522
16.272726	634.557243	13.559539
16.349078	643.753432	13.564557
16.419700	640.690707	13.569575
16.319753	641.561268	13.574592
16.319503	639.847585	13.579610
16.510810	644.794114	13.584627
16.605285	639.114775	13.589645
16.370286	647.674660	13.594663
16.240253	644.397033	13.599680
16.146657	645.171934	13.604698
16.435835	642.851478	13.609715
16.001548	643.335455	13.614733
16.512566	644.590554	13.619751
16.480596	636.652504	13.624768
16.371142	645.852377	13.629786
16.056790	643.449170	13.634803
16.616634	652.402834	13.639821
16.712932	663.378886	13.644839
16.870162	668.952397	13.649856
16.549360	667.266530	13.654874
16.582736	663.477482	13.659891
16.842370	658.488762	13.664909
16.309035	670.298123	13.669927
16.833446	663.362145	13.674944
16.429247	672.901401	13.679962
16.822420	669.233051	13.684979
17.040066	666.163210	13.689997
16.585332	663.516779	13.695015
16.616451	668.942673	13.700032
16.592612	668.463377	13.705050
16.780302	662.264608	13.710067
17.054279	667.270852	13.715085
16.895383	660.387616	13.720103
16.817550	654.211257	13.725120
16.735062	661.832256	13.730138
16.410362	666.019720	13.735155
16.840092	668.729623	13.740173
16.512201	667.972631	13.745191
16.906407	658.178945	13.750208
16.778826	662.815381	13.755226
16.723414	666.717930	13.760243
16.658014	664.951275	13.765261
16.697406	670.713540	13.770279
17.204894	670.697450	13.775296
17.125307	671.022066	13.780314
16.806772	669.929114	13.785331
16.800545	674.612928	13.790349
16.808105	675.870679	13.795367
17.061065	676.111962	13.800384
17.087537	687.625899	13.805402
17.279181	689.334655	13.810419
17.668580	684.029089	13.815437
17.345229	674.615348	13.820455
17.077619	660.355274	13.825472
16.938849	655.744152	13.830490
17.210458	669.545648	13.835507
17.360541	661.421457	13.840525
16.974025	664.015459	13.845543
17.184896	654.408104	13.850560
16.934190	662.755855	13.855578
16.924914	667.768333	13.860595
17.281768	679.682089	13.865613
17.233822	693.867859	13.870631
17.647991	687.955699	13.875648
17.258178	685.176086	13.880666
17.367264	686.389630	13.885683
17.275669	677.179636	13.890701
17.380172	686.917397	13.895719
17.488659	683.132430	13.900736
17.607995	694.830722	13.905754
17.423351	678.326646	13.910771
17.341816	666.732550	13.915789
17.339337	680.374764	13.920807
17.285419	683.425050	13.925824
17.503299	689.077483	13.930842
17.424614	678.407552	13.935859
17.646839	679.003900	13.940877
17.557744	687.231830	13.945895
17.605776	683.620370	13.950912
17.640307	684.144960	13.955930
17.756882	688.544580	13.960947
17.618840	678.843219	13.965965
17.271587	684.968633	13.970983
17.479094	690.638460	13.976000
17.503451	690.142191	13.981018
17.312153	695.921448	13.986035
17.751582	686.076526	13.991053
17.504922	691.457317	13.996071
17.524336	689.948843	14.001088
17.536456	694.052315	14.006106
17.348713	691.866064	14.011123
17.619051	675.303775	14.016141
17.159182	687.196380	14.021159
17.890383	687.874423	14.026176
17.582412	693.217425	14.031194
17.760966	710.637235	14.036211
17.793169	707.911828	14.041229
17.605935	714.536182	14.046247
17.862379	713.366328	14.051264
17.940330	711.034571	14.056282
17.717392	711.495110	14.061299
18.188218	712.582910	14.066317
17.878382	721.441649	14.071335
17.987448	706.668472	14.076352
18.272136	712.906936	14.081370
18.064730	715.214292	14.086387
18.288855	700.470540	14.091405
17.980949	709.316351	14.096423
17.937031	706.041083	14.101440
18.257280	701.847614	14.106458
17.499385	709.097283	14.111475
17.913759	713.677753	14.116493
17.797374	710.451635	14.121511
17.869841	713.744171	14.126528
17.836467	709.255476	14.131546
17.546821	706.797922	14.136563
17.961679	709.554327	14.141581
18.067768	727.020149	14.146599
18.257472	723.850510	14.151616
18.328201	715.233739	14.156634
18.242793	719.077856	14.161651
18.425580	731.665665	14.166669
18.602582	733.812191	14.171687
18.427443	731.204266	14.176704
18.426786	720.474826	14.181722
18.178044	718.477944	14.186739
18.535305	716.121632	14.191757
18.210932	726.273315	14.196775
18.154936	726.212419	14.201792
18.590782	728.665769	14.206810
18.421461	729.594471	14.211827
18.332403	722.788697	14.216845
18.419771	735.599641	14.221863
18.110244	727.812058	14.226880
18.480713	726.820103	14.231898
18.565985	733.992151	14.236915
18.800724	729.651048	14.241933
18.748392	731.236854	14.246951
18.684277	731.600085	14.251968
18.504534	734.354400	14.256986
18.234356	732.919412	14.262003
18.440634	730.151121	14.267021
18.229954	739.859091	14.272039
18.496243	730.328270	14.277056
18.161039	735.214794	14.282074
18.253739	733.089013	14.287091
18.381285	731.787754	14.292109
18.623584	742.027936	14.297127
18.719109	754.979630	14.302144
18.777316	751.319237	14.307162
18.979115	765.204257	14.312179
18.892794	749.505288	14.317197
18.761086	753.845755	14.322215
18.730706	756.617843	14.327232
19.009051	753.320792	14.332250
18.908525	761.115050	14.337267
18.582902	759.874879	14.342285
18.544208	758.119835	14.347303
18.462799	759.094809	14.352320
19.056214	750.712210	14.357338
18.579187	762.724297	14.362355
19.123034	761.377154	14.367373
18.524928	762.959577	14.372391
18.807072	760.823231	14.377408
19.096066	760.803293	14.382426
18.977338	770.597946	14.387443
18.810695	763.390839	14.392461
18.496048	771.612902	14.397479
19.078147	777.956556	14.402496
19.608817	781.382885	14.407514
19.076424	778.685414	14.412531
19.086937	782.584036	14.417549
19.231922	778.032841	14.422567
19.083186	784.376681	14.427584
19.441617	790.581601	14.432602
19.092000	789.673356	14.437619
19.385317	781.435294	14.442637
19.544703	783.130147	14.447655
19.171533	766.715300	14.452672
19.106196	761.401619	14.457690
19.067359	775.958409	14.462707
19.579678	781.896378	14.467725
19.652335	779.682196	14.472743
19.357553	786.206561	14.477760
19.478377	760.313970	14.482778
19.220345	772.194140	14.487795
19.079436	771.859296	14.492813
19.369164	776.995658	14.497831
19.224461	779.760303	14.502848
19.553786	782.419588	14.507866
19.471691	790.962046	14.512883
19.349511	787.572720	14.517901
19.724618	790.559383	14.522919
19.269413	783.069003	14.527936
19.214807	787.066124	14.532954
18.998100	786.604230	14.537971
19.272822	786.491842	14.542989
19.395514	789.773417	14.548007
19.461361	796.263726	14.553024
19.701541	794.932303	14.558042
19.767094	800.728405	14.563059
19.851746	794.397315	14.568077
19.847922	795.129845	14.573095
19.641010	791.529655	14.578112
19.283803	781.224909	14.583130
19.724481	798.809115	14.588147
19.778532	812.436317	14.593165
19.815104	812.727071	14.598183
20.048998	814.994132	14.603200
20.135154	807.791828	14.608218
19.913402	800.747916	14.613235
19.725816	793.540902	14.618253
20.031252	798.463392	14.623271
19.497787	801.326438	14.628288
19.872276	811.959477	14.633306
20.046571	813.752994	14.638323
20.108076	813.115243	14.643341
20.127829	808.151207	14.648359
19.943836	818.546165	14.653376
20.103506	800.868090	14.658394
19.803952	817.150653	14.663411
20.118146	810.540829	14.668429
20.393027	803.918194	14.673447
20.310676	804.211684	14.678464
20.369508	799.516112	14.683482
19.822834	805.073032	14.688499
19.794318	813.733388	14.693517
19.836998	811.637475	14.698535
20.004172	809.509557	14.703552
20.177825	806.392894	14.708570
20.700007	816.330774	14.713587
20.570979	807.615676	14.718605
20.302608	813.886637	14.723623
20.189369	816.119386	14.728640
20.341229	807.865468	14.733658
20.003216	807.466640	14.738675
20.435415	796.493041	14.743693
20.692837	795.726960	14.748711
20.424956	808.069420	14.753728
20.602681	805.356054	14.758746
20.374125	811.917452	14.763763
20.066891	807.231537	14.768781
20.323204	801.416499	14.773799
20.332958	804.056117	14.778816
20.458307	803.518876	14.783834
20.308518	803.418936	14.788851
19.954759	812.713736	14.793869
20.336124	802.331853	14.798887
20.387772	815.422963	14.803904
20.454161	823.822401	14.808922
20.485767	835.540757	14.813939
20.603292	834.626047	14.818957
20.564718	827.714546	14.823975
20.426203	831.989821	14.828992
20.816155	827.088058	14.834010
20.697580	828.239231	14.839027
20.276417	829.806733	14.844045
20.498221	822.062611	14.849063
20.501316	830.326745	14.854080
20.913791	832.092647	14.859098
20.868098	833.649027	14.864115
20.647564	828.441538	14.869133
20.768360	826.753171	14.874151
20.735027	831.797842	14.879168
20.832425	827.329781	14.884186
20.906897	820.631048	14.889203
20.841008	834.157025	14.894221
21.507380	828.183462	14.899239
20.757860	834.043364	14.904256
20.777822	836.782380	14.909274
20.826841	830.557808	14.914291
21.065001	841.603398	14.919309
21.148275	844.654441	14.924327
20.854341	856.959967	14.929344
21.340729	848.095384	14.934362
21.190765	845.991593	14.939379
21.174250	851.592212	14.944397
21.282383	848.305867	14.949415
20.883445	847.944926	14.954432
21.036561	850.855711	14.959450
21.238220	847.289725	14.964467
20.957056	848.797563	14.969485
21.402519	842.716383	14.974503
21.165462	856.022881	14.979520
21.297112	847.585904	14.984538
21.170566	848.653115	14.989555
20.995009	846.234581	14.994573
21.545296	850.399462	14.999591
21.463796	855.827168	15.004608
21.390555	844.736580	15.009626
21.240801	850.547286	15.014643
21.284830	850.243605	15.019661
21.473110	842.447890	15.024679
21.203706	845.866259	15.029696
21.036260	848.596588	15.034714
21.214951	851.004789	15.039731
21.173016	863.207970	15.044749
21.411566	869.201215	15.049767
21.654823	874.758240	15.054784
22.010408	878.331765	15.059802
21.971178	873.585171	15.064819
21.803141	881.983268	15.069837
21.843167	862.117913	15.074855
21.606237	861.491912	15.079872
21.545364	855.369645	15.084890
21.703137	862.003452	15.089907
21.628556	874.962784	15.094925
21.456725	867.440871	15.099943
21.312497	873.739860	15.104960
21.048662	879.912312	15.109978
21.499040	878.958399	15.114995
21.848858	880.390089	15.120013
21.692863	872.824684	15.125031
21.735772	883.948036	15.130048
22.291715	885.568534	15.135066
22.398632	870.823956	15.140083
22.001921	875.622267	15.145101
22.182734	867.376436	15.150119
22.090081	868.182758	15.155136
22.291494	860.195648	15.160154
22.529073	871.553763	15.165171
22.266397	866.428562	15.170189
22.281635	866.006290	15.175207
22.199662	861.695532	15.180224
22.302220	871.269600	15.185242
22.251159	858.130644	15.190259
22.167657	865.212261	15.195277
22.343343	854.398481	15.200295
22.221224	863.063967	15.205312
22.121604	869.258182	15.210330
22.374988	867.381915	15.215347
22.064125	868.237990	15.220365
22.145491	859.291298	15.225383
22.347017	870.096464	15.230400
21.916083	866.622655	15.235418
22.131634	860.062883	15.240435
21.963922	866.100447	15.245453
22.350304	860.224114	15.250471
22.250962	868.425322	15.255488
22.008828	871.795270	15.260506
22.458840	862.390404	15.265523
22.383826	868.309397	15.270541
22.495936	865.189683	15.275559
22.336207	879.623372	15.280576
22.560532	882.870206	15.285594
22.961110	884.290837	15.290611
22.839423	879.484498	15.295629
22.531129	860.667428	15.300647
22.518322	860.347350	15.305664
22.552823	869.054724	15.310682
22.915709	874.056651	15.315699
22.877417	871.067647	15.320717
22.760159	861.034756	15.325735
22.714192	862.925686	15.330752
22.366832	864.756248	15.335770
22.608757	870.199874	15.340787
22.439388	883.183437	15.345805
22.714194	886.548640	15.350823
22.680444	890.290080	15.355840
23.091071	888.067445	15.360858
23.209289	888.121431	15.365875
22.556013	891.883591	15.370893
23.085984	883.908430	15.375911
23.008886	887.369447	15.380928
22.686292	883.260245	15.385946
22.940773	875.561503	15.390963
23.098092	889.302071	15.395981
23.156101	891.170505	15.400999
23.323271	881.150121	15.406016
23.060085	883.238971	15.411034
23.205823	881.250078	15.416051
22.938045	887.394744	15.421069
22.593476	879.795581	15.426087
22.978652	889.369836	15.431104
22.912208	893.747511	15.436122
23.211241	886.912807	15.441139
22.815923	892.553483	15.446157
23.004231	900.946599	15.451175
23.273921	908.989385	15.456192
23.289945	912.338081	15.461210
23.346698	907.955221	15.466227
23.565190	911.117764	15.471245
23.510865	907.070926	15.476263
23.614216	912.709705	15.481280
23.769740	914.869064	15.486298
23.449935	913.302936	15.491315
23.584022	905.979523	15.496333
23.786194	899.895178	15.501351
23.668227	886.791864	15.506368
23.547121	892.146856	15.511386
23.620080	885.271614	15.516403
23.318684	889.625910	15.521421
23.283871	885.235222	15.526439
23.615733	892.454145	15.531456
23.491381	898.743737	15.536474
23.777535	900.358906	15.541491
23.452285	907.329859	15.546509
23.503197	906.081544	15.551527
23.636194	912.479392	15.556544
23.609889	909.236058	15.561562
23.526641	905.124298	15.566579
23.386894	911.217481	15.571597
23.461906	911.562210	15.576615
23.861164	906.438076	15.581632
23.944114	910.994461	15.586650
23.892298	902.144222	15.591667
23.795227	915.845525	15.596685
23.808940	908.430402	15.601703
23.862056	905.338800	15.606720
23.713316	923.649200	15.611738
24.385721	915.247915	15.616755
23.974952	923.150506	15.621773
24.049836	924.606071	15.626791
24.252660	921.920337	15.631808
24.084089	914.072856	15.636826
24.217065	909.400425	15.641843
23.927990	912.831336	15.646861
24.008770	922.582388	15.651879
24.320706	926.273169	15.656896
24.127012	928.922391	15.661914
24.372258	931.575855	15.666931
24.419180	940.445428	15.671949
24.275619	934.506417	15.676967
24.665311	929.926551	15.681984
24.225455	926.334201	15.687002
24.202110	919.309842	15.692019
24.505268	925.810587	15.697037
24.692714	923.111468	15.702055
24.433655	912.668290	15.707072
24.178180	910.230633	15.712090
24.528218	913.369539	15.717107
24.264895	929.192138	15.722125
24.584291	924.162482	15.727143
24.650096	918.345510	15.732160
24.435189	932.005213	15.737178
24.701851	924.310865	15.742195
24.507199	924.173729	15.747213
24.337882	930.211564	15.752231
24.461149	928.074689	15.757248
24.608723	924.981000	15.762266
24.647330	922.484932	15.767283
24.513510	916.938876	15.772301
24.574571	927.447218	15.777319
24.371636	929.558250	15.782336
24.511516	929.457390	15.787354
24.772332	918.923799	15.792371
24.449137	923.063752	15.797389
25.036283	947.987615	15.802407
24.848390	943.093739	15.807424
24.985704	948.124496	15.812442
25.011586	944.368113	15.817459
25.322042	946.320321	15.822477
24.938035	946.212667	15.827495
25.322336	948.784524	15.832512
25.151492	944.626435	15.837530
25.240667	929.894038	15.842547
24.673275	926.211094	15.847565
24.957396	948.351449	15.852583
25.346675	943.317219	15.857600
25.060075	948.420289	15.862618
25.200034	947.735606	15.867635
25.125950	948.371786	15.872653
24.900462	958.404066	15.877671
25.147114	954.187283	15.882688
24.955622	956.063013	15.887706
24.929965	943.617456	15.892723
25.179735	950.688242	15.897741
25.057216	954.165811	15.902759
25.293959	951.389586	15.907776
25.129611	952.402730	15.912794
24.856371	955.790160	15.917811
25.394953	967.360242	15.922829
25.328748	967.840566	15.927847
25.937221	966.786297	15.932864
25.765203	977.794851	15.937882
25.799606	970.887710	15.942899
25.734050	947.841938	15.947917
25.372612	948.327203	15.952935
25.445794	949.981846	15.957952
25.631629	965.037129	15.962970
25.733104	965.242042	15.967987
25.679958	966.528200	15.973005
25.508307	976.163952	15.978023
25.721541	962.920655	15.983040
25.777452	973.474007	15.988058
25.707043	975.949410	15.993075
25.674751	963.523807	15.998093
25.913398	965.061173	16.003111
25.958230	962.725072	16.008128
25.770516	971.574389	16.013146
25.913049	966.382913	16.018163
25.967095	960.577225	16.023181
25.689772	971.273975	16.028199
26.088230	961.776101	16.033216
25.769978	962.008495	16.038234
25.502670	959.512714	16.043251
25.591661	969.085791	16.048269
25.830705	976.025717	16.053287
26.023361	983.638728	16.058304
25.947509	984.603382	16.063322
26.174290	985.085425	16.068339
26.271452	984.940723	16.073357
26.205954	987.210240	16.078375
26.310763	985.448610	16.083392
26.140714	989.956046	16.088410
26.558064	992.898297	16.093427
26.605498	975.313261	16.098445
26.262302	990.813844	16.103463
26.488231	982.526222	16.108480
26.351869	995.523663	16.113498
26.457537	989.908740	16.118515
26.914157	982.910611	16.123533
26.701392	984.802278	16.128551
26.664896	978.433182	16.133568
26.347673	971.691238	16.138586
26.177184	968.956324	16.143603
26.119615	972.250220	16.148621
26.009998	978.774226	16.153639
26.567869	972.931116	16.158656
26.235418	981.900800	16.163674
26.336553	982.358226	16.168691
26.451456	982.633631	16.173709
26.801610	994.737986	16.178727
27.454591	1002.553884	16.183744
27.000489	987.476845	16.188762
26.491022	986.325240	16.193779
26.903608	989.179871	16.198797
26.710747	988.234586	16.203815
27.027743	984.379222	16.208832
26.959150	987.068935	16.213850
26.440699	985.934507	16.218867
27.253919	991.690000	16.223885
26.523407	1005.004012	16.228903
27.023889	1005.594917	16.233920
27.273516	1013.385260	16.238938
27.349978	1009.762996	16.243955
27.361470	996.746740	16.248973
26.962593	994.101029	16.253991
27.022169	980.013815	16.259008
27.066563	979.836304	16.264026
27.115072	1000.921523	16.269043
27.340969	1000.608458	16.274061
26.975813	1003.606273	16.279079
27.247109	1014.432222	16.284096
27.355083	1007.198038	16.289114
27.150592	1007.927106	16.294131
27.389679	1009.442318	16.299149
27.523490	1012.722202	16.304167
27.484023	1001.610478	16.309184
27.357152	1003.103774	16.314202
27.266942	1012.909898	16.319219
27.588553	998.545191	16.324237
27.086244	1000.810137	16.329255
27.401126	1005.245231	16.334272
27.495590	1011.781656	16.339290
27.368141	1003.104085	16.344307
27.639909	997.172970	16.349325
27.495817	1013.447286	16.354343
27.305690	1006.818082	16.359360
27.865013	1004.919413	16.364378
27.563255	1006.992193	16.369395
27.658337	1005.238386	16.374413
27.303104	1006.341211	16.379431
27.757082	1011.897029	16.384448
27.978990	1029.395607	16.389466
27.801381	1025.939128	16.394483
28.219978	1024.469458	16.399501
28.060233	1028.454602	16.404519
27.801322	1010.011529	16.409536
27.882704	1021.340412	16.414554
27.700476	1023.703847	16.419571
28.140824	1032.158767	16.424589
28.152023	1025.498210	16.429607
28.154579	1017.317933	16.434624
28.298198	1020.429037	16.439642
27.990367	1028.236754	16.444659
28.414635	1014.357814	16.449677
28.081552	1021.806549	16.454695
28.072502	1016.108494	16.459712
28.224733	1022.083674	16.464730
28.151154	1022.776581	16.469747
28.034126	1031.936809	16.474765
27.948442	1022.006206	16.479783
28.393109	1025.244005	16.484800
28.186181	1019.945980	16.489818
28.349123	1026.298183	16.494835
28.583320	1016.655444	16.499853
28.589935	1025.146334	16.504871
28.198556	1021.603220	16.509888
28.471477	1011.231789	16.514906
28.221400	1018.929525	16.519923
28.211208	1018.293463	16.524941
28.136743	1034.222448	16.529959
28.417279	1026.144051	16.534976
29.038634	1040.591957	16.539994
29.046111	1048.214893	16.545011
28.865208	1031.896095	16.550029
28.551786	1025.024153	16.555047
28.842604	1029.295746	16.560064
29.060142	1026.257417	16.565082
28.497104	1024.101156	16.570099
28.893516	1019.990426	16.575117
28.946725	1027.827135	16.580135
29.040217	1023.700454	16.585152
28.988211	1011.164279	16.590170
28.429927	1026.641578	16.595187
28.568523	1020.352500	16.600205
28.953584	1037.020969	16.605223
29.184389	1038.221897	16.610240
29.104508	1033.140769	16.615258
29.197831	1033.410068	16.620275
28.955819	1038.654542	16.625293
28.684424	1041.546248	16.630311
29.404650	1041.613801	16.635328
29.361626	1040.607316	16.640346
29.234545	1044.227622	16.645363
29.098544	1035.128496	16.650381
29.081815	1040.085435	16.655399
29.039017	1048.243209	16.660416
29.434203	1038.679532	16.665434
29.286464	1043.439123	16.670451
29.538366	1047.114031	16.675469
29.438463	1045.317996	16.680487
29.182607	1042.558494	16.685504
29.280170	1046.317390	16.690522
29.195796	1040.817245	16.695539
29.500031	1037.276275	16.700557
29.185115	1050.913771	16.705575
29.079668	1055.717273	16.710592
29.574255	1065.334548	16.715610
29.597271	1069.445878	16.720627
29.796081	1064.971435	16.725645
29.404441	1065.792759	16.730663
29.612318	1061.348463	16.735680
29.927499	1060.491329	16.740698
29.365225	1065.990798	16.745715
30.101392	1063.461841	16.750733
29.792837	1056.254620	16.755751
29.782274	1065.335173	16.760768
29.852782	1067.640329	16.765786
29.748588	1062.884865	16.770803
30.162533	1061.112965	16.775821
29.683386	1069.613236	16.780839
29.879246	1060.781159	16.785856
29.774422	1072.031770	16.790874
30.016460	1082.183828	16.795891
30.633474	1081.175560	16.800909
30.560322	1075.670501	16.805927
30.423418	1068.161999	16.810944
29.996500	1058.540120	16.815962
29.970468	1063.511137	16.820979
30.075558	1059.483626	16.825997
30.187551	1079.047449	16.831015
30.146276	1080.098241	16.836032
30.458889	1076.899936	16.841050
30.115597	1083.387781	16.846067
30.300891	1086.284128	16.851085
30.380804	1086.877402	16.856103
30.019088	1084.266917	16.861120
30.492418	1073.785353	16.866138
30.315180	1081.336078	16.871155
30.169510	1080.673771	16.876173
30.158386	1082.114338	16.881191
30.353502	1089.304140	16.886208
30.610965	1100.665618	16.891226
30.817799	1101.728274	16.896243
31.088644	1100.433080	16.901261
30.987917	1081.476162	16.906279
30.799300	1090.625475	16.911296
30.875276	1078.577404	16.916314
30.848892	1079.124113	16.921331
30.854599	1068.273553	16.926349
31.024123	1068.518365	16.931367
30.911756	1077.971375	16.936384
31.045513	1067.258667	16.941402
30.819825	1079.386466	16.946419
31.060782	1077.171290	16.951437
31.127563	1073.683062	16.956455
30.896649	1079.806276	16.961472
30.807869	1071.577079	16.966490
31.003706	1077.965204	16.971507
31.073224	1089.731472	16.976525
31.350197	1099.259572	16.981543
31.166978	1102.528874	16.986560
31.534115	1097.141447	16.991578
31.003280	1091.256369	16.996595
31.029208	1102.581315	17.001613
31.237566	1091.623451	17.006631
30.968641	1104.313411	17.011648
30.976874	1092.471535	17.016666
30.910664	1110.693539	17.021683
31.242473	1105.223249	17.026701
31.307943	1095.379523	17.031719
31.070450	1094.573723	17.036736
31.298472	1104.125227	17.041754
31.179557	1121.544418	17.046771
31.528583	1117.330593	17.051789
31.490687	1117.178516	17.056807
31.548292	1111.952885	17.061824
31.616458	1111.676999	17.066842
31.853098	1113.823753	17.071859
31.764073	1110.785804	17.076877
32.073411	1107.303985	17.081895
32.075557	1115.972337	17.086912
31.937482	1113.153460	17.091930
31.773436	1120.389728	17.096947
31.546427	1108.657049	17.101965
31.546603	1106.091200	17.106983
31.323273	1104.740404	17.112000
31.596299	1111.905463	17.117018
31.960207	1129.647114	17.122035
32.034518	1130.544215	17.127053
32.284314	1123.265813	17.132071
32.291024	1127.079897	17.137088
32.442378	1116.437002	17.142106
32.466721	1122.810818	17.147123
32.637441	1127.934255	17.152141
32.446159	1110.354695	17.157159
32.221252	1108.306721	17.162176
32.466385	1107.148071	17.167194
32.466541	1099.921169	17.172211
32.278819	1098.088310	17.177229
32.314117	1100.291656	17.182247
32.357899	1093.648092	17.187264
32.632079	1091.882170	17.192282
32.674869	1106.243488	17.197299
32.354848	1111.272914	17.202317
32.350139	1106.937444	17.207335
32.741089	1122.528962	17.212352
32.580627	1116.400020	17.217370
32.714947	1123.583523	17.222387
32.292384	1130.459263	17.227405
33.081468	1116.151063	17.232423
33.111696	1125.503003	17.237440
32.782581	1111.962189	17.242458
32.597196	1115.926098	17.247475
32.226704	1118.464021	17.252493
32.502489	1117.335312	17.257511
32.559326	1119.629980	17.262528
32.594462	1120.018791	17.267546
32.864854	1127.540866	17.272563
32.499399	1124.918334	17.277581
32.702145	1119.203050	17.282599
32.964838	1145.970180	17.287616
33.089109	1143.119920	17.292634
33.151400	1145.618867	17.297651
33.464273	1146.399932	17.302669
33.158779	1143.316786	17.307687
32.940236	1153.543752	17.312704
33.204202	1144.426478	17.317722
33.447708	1143.533163	17.322739
33.267569	1141.920023	17.327757
33.366021	1140.699002	17.332775
33.496288	1152.572617	17.337792
33.544947	1139.806087	17.342810
33.256256	1145.433396	17.347827
33.158857	1147.600605	17.352845
33.674964	1144.758764	17.357863
33.401999	1155.051008	17.362880
33.519855	1147.079934	17.367898
33.425172	1136.547917	17.372915
33.532150	1143.707283	17.377933
33.579277	1139.777140	17.382951
33.282149	1141.760852	17.387968
33.516094	1144.387706	17.392986
33.703654	1153.017740	17.398003
33.875389	1166.156682	17.403021
34.090743	1166.858258	17.408039
33.621108	1161.869334	17.413056
33.893543	1171.934661	17.418074
33.959864	1174.922129	17.423091
33.581604	1174.182423	17.428109
33.733994	1165.959815	17.433127
34.042059	1168.022872	17.438144
34.215991	1168.434255	17.443162
34.273373	1169.425511	17.448179
34.082653	1171.020279	17.453197
33.905575	1161.148008	17.458215
33.705154	1164.836561	17.463232
34.037916	1165.803876	17.468250
34.273630	1167.887666	17.473267
33.841027	1168.548116	17.478285
34.333595	1170.475151	17.483303
34.419963	1191.927083	17.488320
34.514330	1199.946806	17.493338
34.596067	1195.399041	17.498355
34.514904	1187.746112	17.503373
34.732088	1183.505462	17.508391
34.315530	1180.714154	17.513408
34.613687	1185.284440	17.518426
34.407390	1196.875974	17.523443
34.763389	1191.550212	17.528461
34.640824	1186.986922	17.533479
34.647961	1185.458227	17.538496
34.387898	1191.314621	17.543514
34.729252	1179.162048	17.548531
34.720315	1187.769045	17.553549
35.134361	1181.970350	17.558567
34.758499	1190.536647	17.563584
34.687520	1187.306529	17.568602
34.773894	1176.904087	17.573619
34.521588	1187.546579	17.578637
34.826293	1181.373592	17.583655
34.848429	1181.262660	17.588672
34.477183	1195.770563	17.593690
34.904391	1199.765344	17.598707
35.099696	1201.883830	17.603725
35.061566	1207.970761	17.608743
35.370380	1199.992023	17.613760
35.189640	1204.491710	17.618778
35.449136	1198.123787	17.623795
35.204112	1207.237761	17.628813
35.251272	1200.464244	17.633831
35.241142	1203.978011	17.638848
35.344244	1197.520830	17.643866
35.218913	1199.342103	17.648883
35.163680	1202.446330	17.653901
35.702603	1205.278171	17.658919
35.667308	1206.760381	17.663936
35.250307	1204.849601	17.668954
35.505536	1205.519724	17.673971
35.254890	1202.582661	17.678989
35.691020	1217.375128	17.684007
36.114575	1230.389705	17.689024
35.883188	1220.349133	17.694042
35.907896	1211.250142	17.699059
35.624004	1205.560105	17.704077
35.947086	1208.797934	17.709095
36.027435	1218.782742	17.714112
35.593417	1215.426107	17.719130
35.706104	1225.061904	17.724147
36.117406	1226.894302	17.729165
36.063615	1227.328519	17.734183
36.185615	1220.688507	17.739200
36.091562	1227.273297	17.744218
36.373403	1215.969403	17.749235
36.201766	1220.641244	17.754253
36.263114	1219.258740	17.759271
36.091826	1219.600797	17.764288
36.189608	1219.935676	17.769306
36.379425	1216.150555	17.774323
36.003270	1222.305899	17.779341
35.972327	1214.657762	17.784359
35.983182	1218.944587	17.789376
35.660836	1227.543595	17.794394
36.456444	1233.342936	17.799411
36.550545	1252.796127	17.804429
36.830358	1240.419567	17.809447
37.338853	1240.854600	17.814464
37.109842	1239.738206	17.819482
37.061312	1231.786689	17.824499
36.771666	1226.488858	17.829517
36.854392	1214.622679	17.834535
36.632521	1218.888935	17.839552
36.741312	1220.714783	17.844570
36.896470	1206.959643	17.849587
36.824499	1217.466779	17.854605
36.938756	1209.218530	17.859623
36.892461	1216.458593	17.864640
36.902354	1225.233089	17.869658
36.759448	1219.246544	17.874675
36.885031	1234.936281	17.879693
37.194200	1244.418422	17.884711
37.162620	1239.967183	17.889728
36.736526	1248.970515	17.894746
37.242837	1243.943226	17.899763
37.227282	1243.560453	17.904781
37.237125	1238.544192	17.909799
37.222744	1245.643599	17.914816
37.296343	1243.482862	17.919834
37.522831	1243.721964	17.924851
37.084907	1248.384779	17.929869
37.334343	1238.846844	17.934887
37.432439	1238.771423	17.939904
37.513610	1243.905679	17.944922
37.699645	1232.086519	17.949939
37.399620	1234.935378	17.954957
37.084451	1244.776655	17.959975
37.585978	1243.764269	17.964992
37.448936	1262.164712	17.970010
37.941248	1258.853191	17.975027
37.717499	1260.674014	17.980045
37.843307	1262.664474	17.985063
37.786862	1258.573706	17.990080
37.339977	1259.359458	17.995098
37.588868	1257.108312	18.000115
37.755590	1257.628116	18.005133
37.780125	1255.926294	18.010151
37.955402	1248.952931	18.015168
37.805492	1264.666653	18.020186
38.321661	1276.473955	18.025203
38.322785	1292.956290	18.030221
38.230143	1278.125681	18.035239
38.540809	1268.161633	18.040256
37.977639	1258.731271	18.045274
38.204265	1266.818795	18.050291
37.958285	1272.707736	18.055309
38.033429	1279.212554	18.060327
38.494600	1280.481774	18.065344
38.135761	1273.793531	18.070362
38.436981	1271.609974	18.075379
38.901483	1273.484586	18.080397
38.745672	1276.421450	18.085415
38.848605	1262.396689	18.090432
38.422915	1273.574309	18.095450
38.570956	1271.064309	18.100467
38.375487	1279.157596	18.105485
38.527623	1277.861937	18.110503
38.750034	1273.008229	18.115520
38.841700	1275.319585	18.120538
38.990222	1278.474152	18.125555
38.706299	1282.027408	18.130573
38.720950	1282.356296	18.135591
39.455231	1287.092234	18.140608
39.275776	1288.587429	18.145626
38.935997	1272.842253	18.150643
39.498817	1279.621435	18.155661
38.956716	1277.414545	18.160679
39.302991	1262.275772	18.165696
39.200893	1273.620760	18.170714
39.220682	1282.693542	18.175731
39.166689	1285.027578	18.180749
39.210739	1289.176709	18.185767
39.203919	1289.490005	18.190784
39.432642	1294.241542	18.195802
39.267300	1292.515631	18.200819
39.607645	1287.955981	18.205837
39.449826	1289.990603	18.210855
39.538333	1291.355715	18.215872
39.396654	1296.802393	18.220890
39.522785	1292.591673	18.225907
39.615299	1294.278052	18.230925
39.426801	1295.051979	18.235943
39.883549	1289.571648	18.240960
39.808318	1289.071934	18.245978
39.635929	1285.624058	18.250995
39.712590	1298.071002	18.256013
39.538030	1297.469989	18.261031
39.830782	1309.876986	18.266048
39.867202	1313.257296	18.271066
40.080622	1308.651130	18.276083
40.303308	1318.853674	18.281101
40.226626	1317.833478	18.286119
40.175116	1308.146702	18.291136
39.932524	1322.003518	18.296154
39.965670	1315.689729	18.301171
40.773456	1312.985486	18.306189
40.283431	1317.968856	18.311207
40.225224	1311.202234	18.316224
40.231011	1305.536491	18.321242
40.113982	1318.105124	18.326259
40.433366	1311.443814	18.331277
40.283070	1316.383757	18.336295
40.652633	1311.096874	18.341312
40.177568	1313.515407	18.346330
40.324836	1312.766456	18.351347
40.667921	1306.792577	18.356365
40.535742	1319.524516	18.361383
40.624659	1332.039004	18.366400
40.724826	1334.235435	18.371418
40.899838	1338.269513	18.376435
41.207756	1342.147199	18.381453
40.745925	1337.756612	18.386471
41.104331	1331.916039	18.391488
40.668601	1342.861736	18.396506
40.940643	1330.009797	18.401523
41.117638	1329.865287	18.406541
41.123427	1339.795500	18.411559
41.453588	1331.033897	18.416576
40.917474	1345.053195	18.421594
41.231596	1331.393130	18.426611
41.376465	1335.659118	18.431629
40.882944	1334.378773	18.436647
41.062043	1329.812659	18.441664
40.551262	1335.484074	18.446682
40.921900	1341.084529	18.451699
41.293900	1352.510387	18.456717
41.443032	1355.516550	18.461735
41.338865	1356.892731	18.466752
41.499322	1352.209593	18.471770
41.325240	1357.702360	18.476787
41.696000	1357.290996	18.481805
41.782329	1359.593726	18.486823
41.822045	1344.202813	18.491840
41.762796	1359.609013	18.496858
41.614558	1343.975964	18.501875
41.773716	1343.600701	18.506893
41.535330	1346.474693	18.511911
42.067810	1342.781362	18.516928
41.705781	1357.205910	18.521946
41.965930	1366.433817	18.526963
42.197077	1374.678476	18.531981
42.295870	1377.061319	18.536999
42.603027	1366.009009	18.542016
42.319467	1356.427764	18.547034
42.220467	1340.629261	18.552051
42.587040	1345.390908	18.557069
42.289808	1350.117052	18.562087
42.296527	1343.229856	18.567104
42.451391	1350.801572	18.572122
42.196006	1360.103430	18.577139
42.765540	1358.174733	18.582157
42.735547	1362.944479	18.587175
42.797192	1350.926857	18.592192
42.187461	1349.317467	18.597210
42.090550	1361.826194	18.602227
42.362683	1365.466460	18.607245
42.499536	1368.455603	18.612263
42.773020	1376.662113	18.617280
42.577636	1369.187836	18.622298
42.310071	1368.440354	18.627315
42.652953	1364.801784	18.632333
42.364326	1382.667376	18.637351
42.954367	1387.599369	18.642368
42.857770	1395.633133	18.647386
42.903693	1402.022625	18.652403
43.452750	1401.728667	18.657421
42.951128	1407.663766	18.662439
42.798997	1394.470722	18.667456
42.869188	1399.985431	18.672474
42.693388	1398.437863	18.677491
42.808502	1399.382274	18.682509
43.191452	1411.144136	18.687527
43.535320	1416.221762	18.692544
43.498694	1414.381124	18.697562
43.964797	1412.866158	18.702579
43.834785	1409.932370	18.707597
43.467216	1407.647796	18.712615
43.845738	1403.476649	18.717632
43.787594	1397.865012	18.722650
43.553625	1395.319797	18.727667
43.807943	1392.064241	18.732685
43.808375	1409.932192	18.737703
44.029259	1408.786766	18.742720
43.721331	1399.849922	18.747738
43.979015	1406.960684	18.752755
43.964806	1405.167049	18.757773
44.108729	1415.176784	18.762791
44.105874	1412.046472	18.767808
44.104679	1412.223194	18.772826
43.903442	1408.117065	18.777843
43.792734	1402.696648	18.782861
44.084590	1408.785918	18.787879
44.152730	1403.441796	18.792896
44.288773	1394.161275	18.797914
43.952674	1401.386574	18.802931
44.227020	1401.460436	18.807949
44.323057	1402.944305	18.812967
44.113766	1400.840217	18.817984
44.325774	1421.294563	18.823002
44.423949	1424.488553	18.828019
44.337426	1425.622150	18.833037
44.385025	1420.539998	18.838055
44.743110	1420.058022	18.843072
44.715923	1424.985139	18.848090
44.468801	1427.585949	18.853107
44.466710	1416.944674	18.858125
44.766640	1423.771154	18.863143
45.024554	1422.304380	18.868160
44.556150	1425.056407	18.873178
44.717100	1446.323464	18.878195
44.907181	1446.729183	18.883213
45.040641	1451.164234	18.888231
45.150267	1452.185242	18.893248
45.302111	1450.416243	18.898266
45.170562	1458.461789	18.903283
45.353130	1446.964921	18.908301
45.285275	1449.234864	18.913319
45.088141	1446.964775	18.918336
45.233006	1443.978716	18.923354
44.937257	1450.219449	18.928371
45.191351	1439.721312	18.933389
45.345908	1461.806740	18.938407
45.297833	1466.191163	18.943424
45.612463	1464.567232	18.948442
45.796100	1472.734126	18.953459
45.745552	1460.263681	18.958477
45.784172	1479.552188	18.963495
46.099690	1476.154543	18.968512
46.026542	1477.039907	18.973530
46.047418	1475.177687	18.978547
46.047569	1470.525789	18.983565
46.066639	1473.984570	18.988583
45.961767	1476.765212	18.993600
46.280598	1472.941016	18.998618
46.150776	1465.349192	19.003635
45.861270	1448.415756	19.008653
45.816628	1470.298677	19.013671
46.161253	1467.461395	19.018688
46.163799	1463.575991	19.023706
46.069711	1457.184132	19.028723
46.283740	1457.144308	19.033741
46.266174	1466.339766	19.038759
46.079819	1459.394223	19.043776
46.357585	1453.490426	19.048794
46.238937	1475.915055	19.053811
46.588767	1476.775589	19.058829
46.616035	1486.068218	19.063847
46.578997	1488.469069	19.068864
46.514722	1484.429961	19.073882
46.571268	1491.591008	19.078899
46.614973	1482.327973	19.083917
46.808192	1487.148207	19.088935
46.803397	1483.838302	19.093952
46.788773	1474.325575	19.098970
46.753117	1480.374343	19.103987
46.672686	1488.131076	19.109005
47.086172	1495.261797	19.114023
47.085529	1505.234129	19.119040
47.339684	1508.511148	19.124058
47.242552	1521.884719	19.129075
47.364359	1507.310868	19.134093
47.450101	1508.442896	19.139111
46.963883	1509.622950	19.144128
47.652163	1507.685217	19.149146
47.409776	1515.981578	19.154163
47.558166	1512.360637	19.159181
47.466745	1511.746671	19.164199
47.529947	1515.855003	19.169216
47.467682	1503.522052	19.174234
47.414091	1513.382712	19.179251
47.615915	1507.620110	19.184269
47.639541	1520.135428	19.189287
47.848782	1530.744133	19.194304
47.986576	1532.284629	19.199322
47.915475	1539.547621	19.204339
48.160833	1529.858686	19.209357
48.068739	1531.018403	19.214375
47.922356	1533.464687	19.219392
48.053991	1531.935514	19.224410
48.059632	1535.538410	19.229427
48.061453	1522.415978	19.234445
48.508916	1518.022630	19.239463
47.967258	1533.898568	19.244480
48.678740	1527.027807	19.249498
48.331033	1528.599710	19.254515
48.323595	1528.865769	19.259533
48.521147	1523.526709	19.264551
48.495302	1530.684821	19.269568
48.581672	1524.791865	19.274586
48.568102	1529.413930	19.279603
48.595561	1526.569215	19.284621
48.678892	1523.548542	19.289639
48.380092	1534.810711	19.294656
48.937775	1542.944648	19.299674
49.103527	1544.143117	19.304691
49.292071	1545.066635	19.309709
49.154931	1544.627046	19.314727
48.849505	1521.479020	19.319744
49.303044	1525.242556	19.324762
48.992992	1530.153781	19.329779
49.672465	1536.226928	19.334797
49.378620	1523.257826	19.339815
48.949086	1531.390826	19.344832
49.234194	1531.330468	19.349850
49.669784	1540.856201	19.354867
49.528408	1541.408204	19.359885
49.472205	1535.543754	19.364903
49.684466	1539.903441	19.369920
49.561372	1525.263563	19.374938
49.361247	1537.943119	19.379955
49.812919	1543.518399	19.384973
49.842670	1546.350676	19.389991
49.429242	1535.732348	19.395008
49.353073	1540.307357	19.400026
49.702232	1540.596792	19.405043
49.824380	1540.091587	19.410061
49.757598	1543.844618	19.415079
49.721173	1546.942821	19.420096
49.851294	1538.398457	19.425114
49.774634	1544.595644	19.430131
49.854774	1553.514000	19.435149
49.796015	1563.662673	19.440167
50.201687	1564.419841	19.445184
50.464522	1559.323074	19.450202
50.009602	1565.645434	19.455219
50.065447	1560.744997	19.460237
50.230412	1561.807889	19.465255
49.980792	1561.480487	19.470272
50.448499	1579.231674	19.475290
50.489356	1582.721799	19.480307
50.740382	1589.275086	19.485325
50.849674	1580.926451	19.490343
50.717812	1589.805248	19.495360
51.080844	1577.103069	19.500378
51.004706	1580.545136	19.505395
51.094243	1577.081670	19.510413
50.770071	1578.810861	19.515431
50.788206	1574.736811	19.520448
50.726130	1568.863797	19.525466
50.960033	1578.673420	19.530483
50.932848	1572.693985	19.535501
51.001952	1573.762335	19.540519
50.727326	1575.783617	19.545536
51.345014	1582.970945	19.550554
51.211987	1598.025915	19.555571
51.114562	1593.600619	19.560589
51.297395	1598.899033	19.565607
51.429181	1600.920159	19.570624
51.406840	1600.642578	19.575642
51.482233	1609.864662	19.580659
51.678804	1606.709578	19.585677
51.579918	1598.579542	19.590695
51.681351	1597.828248	19.595712
51.700322	1600.419212	19.600730
51.738537	1606.200898	19.605747
51.680628	1620.846555	19.610765
52.078998	1623.179633	19.615783
51.925182	1627.874053	19.620800
52.079376	1626.117294	19.625818
51.800221	1629.284862	19.630835
52.010663	1631.303212	19.635853
52.311847	1623.893528	19.640871
51.923772	1627.961692	19.645888
52.205924	1619.500917	19.650906
52.475599	1620.181432	19.655923
52.116462	1626.217496	19.660941
52.198927	1621.297119	19.665959
52.112758	1625.564434	19.670976
52.592784	1629.588959	19.675994
52.883886	1638.925799	19.681011
52.525512	1643.219719	19.686029
52.992194	1638.883311	19.691047
52.925678	1642.102983	19.696064
52.978549	1633.318132	19.701082
52.917810	1620.495706	19.706099
52.859736	1620.296273	19.711117
53.043349	1621.258433	19.716135
53.056789	1643.460733	19.721152
53.273217	1640.775929	19.726170
53.239676	1637.249562	19.731187
53.045866	1640.069323	19.736205
53.099510	1634.443362	19.741223
53.125621	1647.333929	19.746240
53.470245	1640.251995	19.751258
53.358611	1635.387081	19.756275
53.196439	1642.900983	19.761293
53.656671	1626.245129	19.766311
53.413179	1641.011217	19.771328
53.645194	1631.093927	19.776346
53.669602	1633.068658	19.781363
53.599354	1635.203296	19.786381
53.646584	1627.015783	19.791399
53.954446	1629.123108	19.796416
53.759884	1626.394997	19.801434
53.958282	1620.658139	19.806451
53.611284	1632.975617	19.811469
53.854987	1640.290624	19.816487
54.098358	1646.561097	19.821504
54.107887	1650.721998	19.826522
54.119394	1655.204490	19.831539
54.300946	1647.680876	19.836557
54.351632	1657.803095	19.841575
54.007238	1659.352402	19.846592
54.144874	1654.808441	19.851610
54.175445	1652.367171	19.856627
54.113679	1647.368255	19.861645
54.612560	1648.104604	19.866663
54.617145	1671.346593	19.871680
54.808189	1681.816209	19.876698
54.826267	1673.797318	19.881715
54.418836	1676.596695	19.886733
54.854774	1671.346710	19.891751
54.855136	1676.957585	19.896768
54.963647	1678.726719	19.901786
55.052990	1679.716183	19.906803
54.962965	1684.425933	19.911821
54.859555	1675.722199	19.916839
54.915760	1680.364999	19.921856
54.734352	1675.476222	19.926874
55.241023	1681.797234	19.931891
55.173059	1685.130749	19.936909
55.703347	1699.792192	19.941927
55.584628	1695.843565	19.946944
55.492059	1693.670775	19.951962
55.548870	1683.635565	19.956979
55.513243	1701.165433	19.961997
55.945817	1690.677231	19.967015
55.264989	1701.222642	19.972032
55.639321	1693.296602	19.977050
55.715944	1693.650563	19.982067
55.382716	1695.520033	19.987085
55.769454	1700.187116	19.992103
55.786628	1708.724026	19.997120
55.684862	1712.334214	20.002138
55.813588	1690.131407	20.007155
55.577896	1707.032855	20.012173
56.205776	1703.059505	20.017191
56.084830	1715.105154	20.022208
56.031056	1716.350437	20.027226
56.523084	1718.833051	20.032243
56.022829	1720.040550	20.037261
56.535418	1706.409260	20.042279
56.412587	1714.958503	20.047296
55.914442	1720.924722	20.052314
56.247875	1722.554698	20.057331
56.539332	1732.260768	20.062349
56.690474	1731.700549	20.067367
56.603378	1739.313258	20.072384
56.667511	1730.450866	20.077402
56.883412	1734.598591	20.082419
56.645112	1732.347498	20.087437
56.667466	1732.021929	20.092455
56.605546	1735.023147	20.097472
57.144904	1749.291890	20.102490
57.152447	1750.587591	20.107507
57.088907	1766.446100	20.112525
57.238404	1762.550375	20.117543
57.103852	1756.496075	20.122560
57.233000	1766.151693	20.127578
57.488224	1766.250626	20.132595
57.112570	1766.403600	20.137613
57.071356	1757.914210	20.142631
57.222441	1776.491236	20.147648
57.953326	1787.312374	20.152666
58.081803	1779.718071	20.157683
57.587533	1789.038409	20.162701
57.914385	1781.394284	20.167719
57.778486	1791.069091	20.172736
57.778033	1785.915420	20.177754
57.912643	1779.519396	20.182771
57.511390	1787.048491	20.187789
57.952918	1793.288164	20.192807
58.340828	1800.325159	20.197824
58.269538	1800.048884	20.202842
58.626731	1799.907873	20.207859
58.562345	1813.185044	20.212877
58.375344	1799.810931	20.217895
58.926775	1800.845226	20.222912
58.691552	1800.130560	20.227930
59.097993	1789.343405	20.232947
58.568308	1788.693520	20.237965
58.511065	1787.468295	20.242983
58.675750	1792.526589	20.248000
58.766984	1800.853191	20.253018
58.598983	1798.427039	20.258035
58.800187	1806.966902	20.263053
58.851301	1797.213388	20.268071
59.039837	1793.257928	20.273088
59.188996	1804.573601	20.278106
59.216438	1798.989539	20.283123
58.883944	1799.164197	20.288141
58.888856	1808.286902	20.293159
59.666448	1806.287895	20.298176
59.225135	1815.700990	20.303194
59.471587	1812.190956	20.308211
59.522003	1822.856123	20.313229
59.439087	1822.105119	20.318247
59.571093	1819.423966	20.323264
59.457056	1815.938498	20.328282
59.711405	1819.505886	20.333299
59.806944	1826.275978	20.338317
59.798499	1814.448843	20.343335
60.204554	1816.193756	20.348352
59.974732	1814.077035	20.353370
59.917892	1809.266660	20.358387
59.919145	1810.105741	20.363405
59.870713	1810.494955	20.368423
60.173021	1820.098395	20.373440
60.282557	1830.937404	20.378458
60.270317	1835.890710	20.383475
60.368063	1833.760857	20.388493
60.340721	1836.428495	20.393511
60.502379	1830.230219	20.398528
60.432203	1838.200107	20.403546
60.399652	1830.551956	20.408563
60.356108	1835.914089	20.413581
60.356082	1840.805533	20.418599
60.945225	1844.658480	20.423616
61.280516	1862.468437	20.428634
61.186032	1852.365167	20.433651
60.726049	1846.317321	20.438669
61.022813	1852.904612	20.443687
61.206050	1856.558820	20.448704
61.131721	1862.572712	20.453722
61.301836	1850.149692	20.458739
60.856514	1857.527883	20.463757
61.218608	1851.658164	20.468775
61.381351	1843.291617	20.473792
61.146417	1855.456096	20.478810
61.093252	1861.892739	20.483827
61.440466	1865.048035	20.488845
61.630761	1879.809899	20.493863
61.485414	1870.970584	20.498880
61.544650	1877.036272	20.503898
61.774611	1880.863097	20.508915
61.402086	1885.212928	20.513933
61.711254	1882.384258	20.518951
61.835590	1895.259710	20.523968
61.766965	1906.110724	20.528986
62.394985	1901.471414	20.534003
62.313810	1900.657018	20.539021
62.220632	1889.436335	20.544039
62.443436	1901.381250	20.549056
62.709285	1906.108237	20.554074
62.508914	1890.397616	20.559091
62.699463	1893.536281	20.564109
63.072891	1893.219168	20.569127
63.197560	1890.255116	20.574144
62.785719	1891.152205	20.579162
62.814741	1884.116157	20.584179
62.807847	1892.912529	20.589197
62.516907	1892.900832	20.594215
63.008901	1889.500881	20.599232
62.597674	1894.301722	20.604250
62.898115	1883.281698	20.609267
62.484892	1896.777349	20.614285
62.727598	1905.253991	20.619303
63.209273	1903.686067	20.624320
63.104222	1914.498574	20.629338
63.448394	1903.869373	20.634355
63.200008	1918.993069	20.639373
63.361809	1917.859966	20.644391
63.947471	1922.922184	20.649408
64.074656	1924.117216	20.654426
63.710287	1904.023319	20.659443
63.792760	1907.860489	20.664461
63.586135	1901.448120	20.669479
63.783452	1907.514411	20.674496
64.028612	1924.126596	20.679514
64.276236	1925.122990	20.684531
64.287902	1920.737434	20.689549
64.101338	1924.648054	20.694567
64.424315	1923.066966	20.699584
64.326279	1926.048591	20.704602
64.386624	1926.903724	20.709619
64.261699	1920.608021	20.714637
64.307248	1927.543730	20.719655
64.718723	1927.233316	20.724672
64.752203	1929.023625	20.729690
65.139859	1920.565218	20.734707
64.765480	1921.768911	20.739725
64.667893	1925.776134	20.744743
64.779857	1926.847300	20.749760
64.878989	1926.011142	20.754778
64.693155	1921.407019	20.759795
64.505959	1923.799747	20.764813
64.281287	1926.548616	20.769831
64.546231	1927.962049	20.774848
64.591881	1938.542818	20.779866
64.891574	1945.057100	20.784883
65.026750	1956.349800	20.789901
65.058870	1968.340228	20.794919
65.490172	1967.281932	20.799936
65.142970	1971.842443	20.804954
65.175743	1969.063105	20.809971
65.262556	1964.435456	20.814989
65.406318	1983.136917	20.820007
65.843326	1986.697991	20.825024
66.055683	1991.972990	20.830042
66.284839	1990.794682	20.835059
66.288494	1981.483973	20.840077
65.896011	1994.310570	20.845095
66.338421	1986.001404	20.850112
66.222614	1996.736737	20.855130
66.395400	1985.392531	20.860147
66.393139	1989.624777	20.865165
66.059065	1983.528877	20.870183
66.676068	1972.311184	20.875200
66.320139	1978.075459	20.880218
66.408884	1983.480158	20.885235
66.704052	1978.955770	20.890253
66.419839	1979.157627	20.895271
67.104037	1993.650178	20.900288
66.967073	2010.789014	20.905306
67.617877	2009.137942	20.910323
67.218717	1995.553709	20.915341
67.047768	1988.962179	20.920359
67.614376	1976.152280	20.925376
67.147015	1977.348362	20.930394
67.180496	1974.862412	20.935411
67.228879	1976.558883	20.940429
67.213052	1993.388499	20.945447
67.419722	1989.733140	20.950464
67.155304	2002.498778	20.955482
67.041948	1993.152630	20.960499
67.526453	1997.274377	20.965517
67.380734	1999.859480	20.970535
67.709518	2007.407554	20.975552
67.766687	2010.557539	20.980570
68.086343	2019.691310	20.985587
68.338613	2007.987563	20.990605
68.249876	2018.018081	20.995623
68.190824	2010.787404	21.000640
68.227444	2024.039538	21.005658
68.164305	2025.623984	21.010675
68.360206	2008.453488	21.015693
68.105690	2017.657718	21.020711
68.179735	2022.537679	21.025728
68.155972	2021.038971	21.030746
68.380320	2013.877783	21.035763
68.111631	2013.379765	21.040781
68.256953	2031.317301	21.045799
68.635287	2037.241840	21.050816
68.804428	2038.963699	21.055834
68.684055	2045.360376	21.060851
68.785177	2042.257948	21.065869
68.741481	2047.064725	21.070887
68.762709	2043.009023	21.075904
68.732978	2059.430594	21.080922
69.361016	2065.060635	21.085939
69.198500	2063.829689	21.090957
69.025099	2061.495862	21.095975
69.390437	2055.795993	21.100992
69.217971	2060.783775	21.106010
69.545359	2068.139580	21.111027
69.323558	2080.097031	21.116045
69.514546	2084.510659	21.121063
69.635086	2090.027210	21.126080
70.051162	2091.224614	21.131098
69.923002	2094.169929	21.136115
70.188168	2094.513480	21.141133
69.854107	2092.652806	21.146151
69.990973	2082.617531	21.151168
69.705303	2086.792935	21.156186
70.083161	2105.858881	21.161203
70.122648	2115.089973	21.166221
70.047266	2106.315391	21.171239
70.385132	2106.612907	21.176256
70.372596	2114.507670	21.181274
70.304555	2115.849880	21.186291
70.688186	2115.890952	21.191309
70.536113	2127.970128	21.196327
70.761708	2130.292303	21.201344
70.848737	2132.506659	21.206362
70.692663	2126.297787	21.211379
70.779039	2130.030251	21.216397
71.109337	2137.770656	21.221415
71.393374	2139.278968	21.226432
71.710100	2146.163074	21.231450
71.247537	2144.795793	21.236467
71.692940	2132.664246	21.241485
71.444801	2158.388915	21.246503
71.604874	2161.150504	21.251520
71.241142	2164.975146	21.256538
71.415300	2154.104011	21.261555
71.262303	2148.579492	21.266573
71.024482	2154.524259	21.271591
72.011794	2160.486574	21.276608
72.208178	2170.359171	21.281626
72.124770	2167.376974	21.286643
72.425118	2167.475197	21.291661
72.277162	2171.745949	21.296679
72.480175	2170.073059	21.301696
72.534384	2163.541087	21.306714
72.605961	2166.092383	21.311731
73.072193	2163.182409	21.316749
72.937482	2167.040825	21.321767
72.711795	2168.808389	21.326784
72.694638	2168.845587	21.331802
72.676842	2173.152882	21.336819
72.759151	2170.485725	21.341837
72.566178	2174.157545	21.346855
72.987616	2158.233107	21.351872
72.907022	2157.958274	21.356890
73.020357	2171.047087	21.361907
73.071967	2161.589957	21.366925
72.878764	2165.722579	21.371943
72.941447	2168.107995	21.376960
73.007525	2182.939946	21.381978
72.858332	2189.470555	21.386995
73.236782	2183.424605	21.392013
73.242506	2184.086275	21.397031
73.262427	2200.812685	21.402048
73.499439	2219.853342	21.407066
73.659320	2217.660119	21.412083
74.035971	2204.740771	21.417101
74.010644	2212.138927	21.422119
73.319330	2209.750010	21.427136
74.066521	2219.937684	21.432154
73.908327	2230.146400	21.437171
74.336173	2229.413691	21.442189
74.023904	2238.677521	21.447207
74.206537	2239.078108	21.452224
74.286862	2228.410895	21.457242
74.123403	2238.674086	21.462259
74.361534	2249.493327	21.467277
74.693079	2248.554694	21.472295
74.773471	2256.349839	21.477312
74.855671	2269.721296	21.482330
74.572958	2272.242557	21.487347
75.251803	2256.887056	21.492365
75.082774	2257.342395	21.497383
75.067823	2264.723177	21.502400
75.005033	2252.566525	21.507418
75.111379	2266.811578	21.512435
75.652368	2285.621932	21.517453
75.811313	2285.732703	21.522471
75.425051	2285.436029	21.527488
75.711169	2275.099684	21.532506
75.751139	2282.939006	21.537523
76.110815	2278.969418	21.542541
75.693384	2283.080170	21.547559
76.128939	2269.716081	21.552576
76.547203	2275.546116	21.557594
76.203742	2272.156242	21.562611
76.223141	2271.332482	21.567629
76.476358	2271.864098	21.572647
76.219525	2270.288042	21.577664
76.471208	2269.399713	21.582682
76.211078	2274.205533	21.587699
76.377879	2263.733129	21.592717
76.548367	2271.113446	21.597735
76.401870	2276.734750	21.602752
76.640922	2279.518777	21.607770
76.450460	2287.993611	21.612787
76.678309	2290.738356	21.617805
76.747494	2301.284116	21.622823
76.400287	2297.049020	21.627840
77.062967	2306.770195	21.632858
77.319585	2321.664117	21.637875
77.532405	2324.755209	21.642893
77.540528	2327.458426	21.647911
77.228917	2333.471547	21.652928
77.630891	2324.859235	21.657946
77.246495	2323.173640	21.662963
77.145954	2329.015035	21.667981
77.290406	2319.208833	21.672999
77.609141	2337.700377	21.678016
77.924869	2336.126694	21.683034
77.697598	2343.187096	21.688051
78.371714	2339.878634	21.693069
78.286993	2349.135497	21.698087
78.262317	2337.487278	21.703104
78.346361	2334.990250	21.708122
78.230825	2341.749217	21.713139
78.160346	2330.644650	21.718157
78.687986	2335.984278	21.723175
78.418456	2332.008495	21.728192
78.766366	2331.487054	21.733210
78.505636	2329.362460	21.738227
78.868185	2329.062814	21.743245
78.551562	2332.697110	21.748263
78.561566	2345.319274	21.753280
78.898254	2353.345973	21.758298
78.564259	2361.369792	21.763315
78.754335	2356.511358	21.768333
78.790823	2358.705207	21.773351
79.005303	2375.581380	21.778368
79.490633	2375.549812	21.783386
79.557468	2370.063586	21.788403
79.615326	2376.117033	21.793421
79.541952	2373.795996	21.798439
79.250989	2387.244576	21.803456
79.849096	2385.686888	21.808474
79.767460	2402.454546	21.813491
79.981606	2409.739755	21.818509
80.251743	2402.094730	21.823527
79.826561	2400.311329	21.828544
79.632247	2403.017672	21.833562
79.960611	2406.106568	21.838579
80.393757	2412.117378	21.843597
80.499078	2415.805924	21.848615
80.784414	2423.938485	21.853632
80.690098	2423.738373	21.858650
80.763261	2429.751584	21.863667
80.873495	2421.263548	21.868685
81.124024	2423.335712	21.873703
80.460515	2425.995181	21.878720
81.001498	2419.412576	21.883738
80.876979	2416.342058	21.888755
81.150332	2436.898477	21.893773
81.445309	2440.071477	21.898791
81.582318	2441.309199	21.903808
81.724610	2441.173240	21.908826
81.663096	2440.141150	21.913843
81.692040	2442.459267	21.918861
81.865228	2438.891087	21.923879
81.604050	2437.867991	21.928896
81.631765	2431.314799	21.933914
81.347457	2443.203324	21.938931
81.463204	2436.090436	21.943949
81.793693	2446.693434	21.948967
81.924737	2462.427584	21.953984
82.338801	2458.938669	21.959002
82.088011	2456.591591	21.964019
82.240533	2455.235825	21.969037
82.480840	2465.571990	21.974055
81.987627	2472.437148	21.979072
82.439050	2479.739096	21.984090
82.454822	2482.535826	21.989107
82.697482	2477.476656	21.994125
82.740570	2478.871024	21.999143
82.684975	2488.016119	22.004160
82.837387	2486.455227	22.009178
82.996350	2509.841538	22.014195
83.117750	2501.042437	22.019213
83.339016	2507.777433	22.024231
83.210930	2511.625423	22.029248
83.670074	2516.104713	22.034266
83.777648	2512.941235	22.039283
83.562773	2510.585402	22.044301
83.364183	2506.443891	22.049319
83.318550	2512.554525	22.054336
83.388028	2515.465983	22.059354
83.851841	2527.067661	22.064371
83.651980	2530.169388	22.069389
84.052750	2534.253801	22.074407
84.123955	2535.848936	22.079424
83.776461	2531.519149	22.084442
83.825430	2541.459087	22.089459
84.186227	2565.631454	22.094477
84.489187	2545.795878	22.099495
84.322964	2541.049676	22.104512
84.790851	2539.376541	22.109530
84.922229	2541.407306	22.114547
84.725374	2544.909381	22.119565
85.244653	2554.608834	22.124583
85.025447	2572.243881	22.129600
85.342144	2567.046919	22.134618
85.418031	2566.548888	22.139635
85.322595	2563.666334	22.144653
85.380675	2558.591695	22.149671
85.340190	2565.092892	22.154688
85.508273	2569.390278	22.159706
85.233908	2562.451695	22.164723
85.692005	2570.317568	22.169741
85.731501	2565.214261	22.174759
85.761525	2576.918226	22.179776
85.947550	2578.252475	22.184794
86.060021	2586.459364	22.189811
85.858615	2587.945459	22.194829
86.524231	2578.392512	22.199847
86.629688	2577.113496	22.204864
86.359683	2579.408743	22.209882
86.059493	2582.219966	22.214899
86.226298	2588.004041	22.219917
86.738847	2596.208610	22.224935
86.622792	2608.910550	22.229952
86.562217	2609.844508	22.234970
86.675461	2603.252688	22.239987
86.847344	2602.730242	22.245005
87.184868	2597.574213	22.250023
87.057221	2596.476666	22.255040
87.411561	2608.780299	22.260058
87.833566	2615.730252	22.265075
87.702550	2614.314469	22.270093
88.078803	2617.853570	22.275111
87.700664	2604.682196	22.280128
87.856056	2597.594632	22.285146
87.446440	2601.843104	22.290163
87.436575	2616.579933	22.295181
88.003856	2613.022950	22.300199
87.820549	2618.710056	22.305216
87.854789	2615.782055	22.310234
87.842954	2620.350479	22.315251
88.049704	2634.109945	22.320269
88.361752	2642.926461	22.325287
88.189805	2654.750291	22.330304
88.475507	2650.416572	22.335322
88.562400	2648.215724	22.340339
88.558181	2650.592684	22.345357
88.903385	2649.535131	22.350375
88.842044	2663.970722	22.355392
88.757694	2666.489557	22.360410
89.014709	2667.796980	22.365427
89.011070	2662.813978	22.370445
89.118541	2656.655415	22.375463
88.809734	2668.352228	22.380480
88.696064	2668.802114	22.385498
89.549582	2677.670054	22.390515
89.451691	2683.328102	22.395533
89.671765	2689.896082	22.400551
89.645344	2688.363015	22.405568
89.654713	2682.803584	22.410586
89.764587	2684.238066	22.415603
89.584197	2700.121906	22.420621
90.049718	2701.283251	22.425639
89.894605	2703.809953	22.430656
89.717948	2708.590267	22.435674
90.295577	2712.782896	22.440691
90.020254	2724.420880	22.445709
90.631570	2728.794474	22.450727
90.777958	2734.805855	22.455744
90.742614	2731.235368	22.460762
90.838073	2734.565726	22.465779
90.692733	2735.074197	22.470797
91.185643	2726.144555	22.475815
90.802212	2736.155079	22.480832
90.964758	2750.893579	22.485850
91.812705	2743.347810	22.490867
91.724051	2743.143657	22.495885
91.969003	2738.655302	22.500903
91.804864	2743.623040	22.505920
91.620286	2743.080344	22.510938
92.071687	2734.652660	22.515955
91.740037	2749.913105	22.520973
91.823144	2744.812425	22.525991
91.958612	2746.154558	22.531008
91.880349	2744.623246	22.536026
92.150826	2745.736059	22.541043
92.242681	2759.055882	22.546061
92.483327	2764.677028	22.551079
92.494000	2761.427599	22.556096
92.298382	2766.501238	22.561114
92.602891	2766.466264	22.566131
92.380817	2760.958622	22.571149
92.701986	2780.835752	22.576167
92.621870	2790.704400	22.581184
92.887023	2793.276144	22.586202
93.074474	2784.504493	22.591219
92.808902	2793.092253	22.596237
93.163053	2794.892687	22.601255
93.402923	2815.751423	22.606272
93.452265	2814.904040	22.611290
93.166697	2814.954624	22.616307
93.036554	2814.567565	22.621325
93.454340	2821.215274	22.626343
93.877382	2835.525090	22.631360
93.970797	2829.264506	22.636378
94.362004	2824.724955	22.641395
94.297373	2837.614726	22.646413
94.468602	2838.629380	22.651431
94.392602	2838.981879	22.656448
94.235155	2836.973697	22.661466
94.309800	2831.056889	22.666483
93.977232	2846.219720	22.671501
94.758339	2863.778213	22.676519
94.655750	2868.139906	22.681536
94.515823	2865.084334	22.686554
94.424140	2864.520858	22.691571
94.983479	2876.461371	22.696589
95.145560	2889.360067	22.701607
94.921480	2888.286984	22.706624
95.325997	2885.137174	22.711642
95.586907	2871.190708	22.716659
95.709867	2873.611019	22.721677
95.325410	2885.657451	22.726695
95.559741	2885.532408	22.731712
95.937509	2900.609940	22.736730
95.917351	2904.933558	22.741747
96.057700	2915.547501	22.746765
96.072434	2902.037005	22.751783
96.109875	2901.904744	22.756800
96.172698	2907.017087	22.761818
96.137524	2904.175592	22.766835
96.147962	2915.933325	22.771853
96.542644	2924.336293	22.776871
96.546012	2926.503807	22.781888
96.633387	2935.317575	22.786906
96.993442	2922.974703	22.791923
96.782152	2932.232636	22.796941
97.104941	2923.443002	22.801959
97.661973	2925.691587	22.806976
96.910438	2924.277707	22.811994
97.657850	2935.923868	22.817011
97.597730	2939.145932	22.822029
97.543176	2938.292626	22.827047
97.693443	2937.625200	22.832064
97.390867	2939.824569	22.837082
97.631373	2937.189478	22.842099
97.748983	2940.263940	22.847117
98.061205	2961.591305	22.852135
98.057775	2962.390141	22.857152
97.897446	2972.555425	22.862170
98.254290	2962.362323	22.867187
98.166573	2972.462648	22.872205
98.473799	2976.205090	22.877223
98.812649	2988.533488	22.882240
98.714047	2994.964987	22.887258
99.186838	2991.466827	22.892275
99.042019	2998.401029	22.897293
99.109145	2997.478278	22.902311
99.089096	2998.162927	22.907328
99.105465	2992.712773	22.912346
99.011899	2994.415661	22.917363
99.594849	2995.934318	22.922381
99.515533	3015.956120	22.927399
99.916282	3014.163996	22.932416
99.591638	3011.749441	22.937434
99.938659	3012.228604	22.942451
100.036191	3019.974071	22.947469
99.636212	3027.771752	22.952487
99.932920	3014.501320	22.957504
99.603666	3018.955148	22.962522
100.078125	3034.147138	22.967539
100.183326	3039.808394	22.972557
100.335413	3042.773354	22.977575
100.290097	3033.277202	22.982592
100.450441	3056.925967	22.987610
100.504117	3051.476300	22.992627
100.828082	3060.016586	22.997645
100.388327	3052.866854	23.002663
100.859358	3068.719032	23.007680
100.713229	3080.195106	23.012698
101.598497	3080.404260	23.017715
101.880308	3064.437637	23.022733
101.821027	3070.042453	23.027751
101.907874	3061.747122	23.032768
101.829617	3069.172809	23.037786
101.926642	3065.319689	23.042803
102.275178	3061.922921	23.047821
102.396567	3058.302717	23.052839
102.462623	3059.734584	23.057856
101.749432	3071.813385	23.062874
102.441759	3063.682585	23.067891
102.059836	3067.639648	23.072909
102.306219	3084.902879	23.077927
102.767097	3087.718775	23.082944
102.466614	3080.799837	23.087962
102.559051	3087.836003	23.092979
102.611147	3093.669662	23.097997
102.534692	3095.139500	23.103015
103.021248	3099.620982	23.108032
103.124797	3114.362654	23.113050
103.122357	3110.187307	23.118067
102.908486	3113.692141	23.123085
103.211376	3132.748761	23.128103
103.402705	3133.772926	23.133120
103.359091	3149.945168	23.138138
103.584586	3146.775844	23.143155
103.831313	3152.879051	23.148173
103.830952	3162.505089	23.153191
103.977769	3164.470399	23.158208
104.109111	3176.007486	23.163226
104.143337	3173.540191	23.168243
104.196905	3172.370208	23.173261
104.583529	3186.234650	23.178279
104.402889	3189.333496	23.183296
104.587095	3193.915730	23.188314
104.802321	3184.561989	23.193331
105.225231	3190.849239	23.198349
104.812568	3197.055124	23.203367
105.139629	3202.625079	23.208384
105.178353	3202.710389	23.213402
105.282769	3203.533474	23.218419
105.314902	3210.171936	23.223437
105.400861	3211.565998	23.228455
105.663371	3213.260810	23.233472
105.833245	3223.204395	23.238490
105.991552	3231.697963	23.243507
106.256447	3226.272168	23.248525
105.974871	3230.914305	23.253543
106.454446	3229.706398	23.258560
105.991506	3221.225164	23.263578
106.298889	3229.168447	23.268595
106.738439	3240.667059	23.273613
106.949959	3240.226796	23.278631
107.087789	3247.555790	23.283648
107.094809	3253.964624	23.288666
106.999846	3246.054158	23.293683
107.139692	3247.001131	23.298701
107.289643	3249.332074	23.303719
107.401951	3247.843639	23.308736
107.423037	3249.424549	23.313754
107.338519	3242.430894	23.318771
107.367616	3257.493577	23.323789
107.322826	3270.670934	23.328807
107.497276	3267.190766	23.333824
107.742609	3272.887089	23.338842
107.717139	3287.191349	23.343859
107.864685	3290.270679	23.348877
107.892507	3305.317818	23.353895
107.941199	3298.508552	23.358912
107.880392	3314.645745	23.363930
108.482463	3319.667936	23.368947
108.629629	3313.032702	23.373965
108.531097	3323.589393	23.378983
108.900922	3327.240103	23.384000
108.920056	3338.283467	23.389018
108.966536	3344.664097	23.394035
109.012329	3339.591151	23.399053
109.517366	3349.476311	23.404071
109.326550	3341.918435	23.409088
109.620247	3353.086338	23.414106
109.669824	3346.216949	23.419123
109.628751	3333.787910	23.424141
109.474037	3359.001078	23.429159
109.760802	3366.502615	23.434176
109.852722	3360.040085	23.439194
110.022056	3361.452740	23.444211
110.221872	3354.067596	23.449229
110.217985	3376.517763	23.454247
110.316717	3383.158545	23.459264
110.484443	3385.862322	23.464282
110.530661	3382.932332	23.469299
111.115468	3385.725824	23.474317
110.697559	3390.853184	23.479335
110.807232	3396.349736	23.484352
111.563748	3405.293111	23.489370
111.228520	3407.971044	23.494387
111.710606	3407.968390	23.499405
111.670508	3413.898567	23.504423
111.513872	3403.826191	23.509440
111.664107	3399.396607	23.514458
112.006929	3417.727707	23.519475
111.972450	3422.255674	23.524493
112.109865	3438.548330	23.529511
112.124072	3432.078936	23.534528
111.996422	3427.534801	23.539546
112.043079	3433.776563	23.544563
112.911584	3433.196135	23.549581
112.445263	3445.981605	23.554599
112.970001	3454.541319	23.559616
112.885086	3456.246060	23.564634
112.990695	3458.328284	23.569651
113.128593	3452.704417	23.574669
113.095885	3462.240966	23.579687
113.172637	3454.688727	23.584704
113.045390	3473.497061	23.589722
113.264620	3476.678884	23.594739
113.549226	3478.887895	23.599757
113.563621	3483.162086	23.604775
113.366541	3494.539046	23.609792
113.747048	3489.672753	23.614810
113.519402	3499.107112	23.619827
114.029828	3503.370360	23.624845
114.075941	3521.820353	23.629863
114.763846	3524.121233	23.634880
114.654967	3522.010726	23.639898
114.449452	3519.252467	23.644915
114.753108	3519.713147	23.649933
114.716400	3532.333949	23.654951
115.021530	3540.321907	23.659968
115.156139	3547.692556	23.664986
115.177775	3557.369035	23.670003
115.649475	3546.302395	23.675021
115.521289	3551.804465	23.680039
115.467249	3538.793409	23.685056
115.250669	3562.226934	23.690074
115.336859	3573.430437	23.695091
115.826244	3577.450796	23.700109
115.689609	3583.815833	23.705127
116.098213	3591.825579	23.710144
116.254686	3596.519544	23.715162
116.287477	3602.488935	23.720179
116.509269	3591.145555	23.725197
116.241235	3597.751989	23.730215
116.510840	3600.468343	23.735232
116.865021	3624.321234	23.740250
116.863216	3625.716368	23.745267
117.094176	3619.560343	23.750285
116.701656	3632.893102	23.755303
117.074183	3619.840824	23.760320
117.012547	3635.277755	23.765338
117.214032	3645.308181	23.770355
117.741905	3642.707154	23.775373
117.488926	3650.201312	23.780391
117.659314	3648.877394	23.785408
117.656745	3662.278867	23.790426
117.663505	3660.229246	23.795443
117.794128	3661.464891	23.800461
118.221964	3679.981864	23.805479
118.385663	3678.567455	23.810496
118.611803	3684.191148	23.815514
118.439186	3688.538691	23.820531
119.184522	3689.113670	23.825549
118.962279	3686.875608	23.830567
119.010668	3690.298691	23.835584
119.469485	3693.257034	23.840602
119.154595	3702.910236	23.845619
119.441833	3701.798526	23.850637
119.333536	3713.701514	23.855655
119.510450	3704.246158	23.860672
119.686485	3701.040251	23.865690
119.970310	3715.520788	23.870707
120.128416	3734.490120	23.875725
120.216713	3734.428840	23.880743
120.339108	3730.742065	23.885760
120.293118	3730.493383	23.890778
120.506850	3737.634011	23.895795
120.851936	3729.231887	23.900813
120.383615	3737.854818	23.905831
120.777648	3741.672280	23.910848
120.484254	3747.458942	23.915866
120.524374	3754.806512	23.920883
121.281393	3761.966720	23.925901
121.165169	3779.242885	23.930919
121.067149	3775.079108	23.935936
121.773897	3775.666412	23.940954
121.538767	3784.868523	23.945971
122.062588	3794.031384	23.950989
121.973474	3794.717347	23.956007
122.212779	3803.526823	23.961024
122.259278	3799.185885	23.966042
122.230218	3808.267551	23.971059
122.206715	3803.669231	23.976077
122.489135	3814.555115	23.981095
122.431918	3824.357639	23.986112
122.588180	3826.706612	23.991130
122.576703	3827.134303	23.996147
122.952780	3828.600025	24.001165
122.795620	3850.134086	24.006183
122.930546	3859.660526	24.011200
123.306387	3850.268810	24.016218
123.439425	3865.924972	24.021235
123.805418	3866.609519	24.026253
123.669889	3862.625156	24.031271
123.846390	3869.613821	24.036288
123.842342	3870.576917	24.041306
123.960417	3869.548346	24.046323
123.828313	3893.780304	24.051341
124.059457	3893.472691	24.056359
124.233932	3897.671557	24.061376
124.615550	3899.821329	24.066394
124.430856	3919.759540	24.071411
124.741820	3926.803042	24.076429
125.186023	3926.945164	24.081447
124.896642	3921.911614	24.086464
125.007030	3920.221423	24.091482
125.275496	3938.069098	24.096499
125.298764	3934.220965	24.101517
125.383651	3943.123989	24.106535
125.458154	3939.223690	24.111552
125.640826	3937.721088	24.116570
125.387582	3961.119807	24.121587
125.725809	3959.826548	24.126605
126.021704	3967.721447	24.131623
126.058581	3976.212179	24.136640
126.593467	3977.167124	24.141658
126.755578	3986.212804	24.146675
127.135387	3983.653719	24.151693
127.370170	3973.295989	24.156711
127.468296	3979.028081	24.161728
127.994240	3969.010087	24.166746
127.297941	3979.186789	24.171763
127.414765	3964.627503	24.176781
127.602337	3968.297251	24.181799
127.650533	3971.256447	24.186816
127.935784	3963.453752	24.191834
127.657537	3976.768972	24.196851
128.116581	3991.074106	24.201869
128.397235	4003.800484	24.206887
128.162617	3999.133981	24.211904
128.639822	3992.516552	24.216922
128.457344	4000.530132	24.221939
128.747315	3992.054405	24.226957
128.640487	3998.228727	24.231975
128.805960	4012.314457	24.236992
128.843768	4005.901153	24.242010
128.785433	4014.517196	24.247027
129.169163	4026.788821	24.252045
129.388096	4036.804124	24.257063
129.246404	4038.508289	24.262080
129.842650	4033.721889	24.267098
129.519196	4041.012555	24.272115
129.699262	4057.987198	24.277133
129.996775	4059.023293	24.282151
130.245669	4060.436242	24.287168
130.558663	4045.906318	24.292186
130.646976	4054.376454	24.297203
130.751857	4077.605941	24.302221
130.996156	4079.871803	24.307239
131.132967	4069.605023	24.312256
131.483506	4073.429328	24.317274
131.174442	4083.365891	24.322291
131.459289	4077.450667	24.327309
131.910069	4080.293545	24.332327
131.674300	4085.831465	24.337344
131.862598	4071.166277	24.342362
131.675551	4077.192145	24.347379
131.779040	4076.266835	24.352397
132.191869	4079.102995	24.357415
132.177764	4095.905903	24.362432
132.539776	4095.817789	24.367450
132.337482	4091.711206	24.372467
132.318215	4094.674612	24.377485
132.106468	4101.348216	24.382503
132.171244	4112.845767	24.387520
132.497017	4123.226394	24.392538
132.633687	4132.916835	24.397555
132.871954	4153.237646	24.402573
133.063671	4146.491012	24.407591
133.178946	4156.847619	24.412608
133.554362	4163.313047	24.417626
133.635786	4168.457571	24.422643
133.992245	4170.286195	24.427661
134.323788	4161.437786	24.432679
134.163384	4169.126061	24.437696
134.357680	4159.146972	24.442714
134.041915	4169.861075	24.447731
134.397912	4173.258451	24.452749
134.914796	4178.619248	24.457767
134.653488	4187.330101	24.462784
135.028158	4187.596679	24.467802
134.809402	4188.823630	24.472819
135.030834	4198.772352	24.477837
135.098503	4205.983251	24.482855
135.116233	4223.690337	24.487872
135.037643	4216.146184	24.492890
135.411164	4229.404304	24.497907
135.482734	4232.448279	24.502925
135.799571	4241.896099	24.507943
135.734163	4252.037855	24.512960
136.027248	4258.740234	24.517978
136.225493	4262.035935	24.522995
135.983114	4275.011221	24.528013
135.945296	4284.498498	24.533031
136.082912	4291.446036	24.538048
136.614851	4301.987204	24.543066
136.717453	4311.392663	24.548083
136.660502	4318.304221	24.553101
137.083453	4328.505709	24.558119
137.206852	4344.002814	24.563136
137.349974	4343.147071	24.568154
138.079821	4360.951739	24.573171
137.819145	4364.543009	24.578189
137.968454	4355.590311	24.583207
138.352069	4355.299985	24.588224
138.531962	4362.802795	24.593242
138.686895	4365.698092	24.598259
138.643658	4377.042185	24.603277
139.058543	4381.573026	24.608295
138.996305	4392.427699	24.613312
139.003727	4388.840756	24.618330
139.230400	4386.393835	24.623347
138.931743	4386.610586	24.628365
139.396665	4396.486788	24.633383
139.525023	4409.341322	24.638400
139.697450	4405.261547	24.643418
139.790683	4404.113717	24.648435
139.635570	4427.728174	24.653453
139.959624	4437.938808	24.658471
139.760182	4431.745358	24.663488
140.154308	4440.805645	24.668506
140.733005	4449.376373	24.673523
140.367741	4459.419737	24.678541
140.852463	4451.301706	24.683559
140.785632	4461.933035	24.688576
141.124175	4460.917451	24.693594
141.373328	4467.402647	24.698611
141.412621	4468.501063	24.703629
141.654935	4464.287297	24.708647
141.501441	4468.622580	24.713664
141.877820	4481.107134	24.718682
141.977145	4484.244677	24.723699
141.721137	4493.456712	24.728717
142.027788	4500.630521	24.733735
142.256131	4517.304539	24.738752
142.433648	4516.522342	24.743770
142.194276	4517.907187	24.748787
142.251647	4516.850154	24.753805
142.804511	4531.980703	24.758823
142.685836	4547.506202	24.763840
142.688929	4540.602564	24.768858
143.016051	4553.669295	24.773875
142.841903	4565.097015	24.778893
143.094475	4562.822794	24.783911
143.480052	4585.788287	24.788928
143.442502	4589.603684	24.793946
143.803654	4581.444863	24.798963
144.110478	4605.814601	24.803981
144.318659	4606.577406	24.808999
144.672008	4618.090321	24.814016
144.829755	4623.279907	24.819034
144.777879	4618.966714	24.824051
144.935607	4626.974949	24.829069
144.895545	4634.104945	24.834087
145.288343	4639.854496	24.839104
145.708785	4629.877817	24.844122
146.113334	4627.311635	24.849139
145.828574	4624.732830	24.854157
146.078751	4625.545913	24.859175
146.264368	4626.321702	24.864192
146.224371	4627.546102	24.869210
146.521117	4631.666132	24.874227
146.174089	4639.857119	24.879245
146.747055	4641.109187	24.884263
146.948551	4646.692829	24.889280
146.949160	4649.889960	24.894298
146.829156	4650.748052	24.899315
147.065379	4664.930593	24.904333
147.167365	4668.951543	24.909351
147.136019	4685.593550	24.914368
147.636796	4673.839918	24.919386
147.532771	4692.778471	24.924403
147.508105	4706.323038	24.929421
147.681659	4701.075157	24.934439
147.746719	4718.431311	24.939456
148.002362	4727.349170	24.944474
148.554707	4736.921559	24.949491
148.094355	4738.451298	24.954509
148.486558	4750.750504	24.959527
148.575314	4764.125949	24.964544
148.506984	4763.423052	24.969562
149.061442	4775.188832	24.974579
148.870972	4792.733191	24.979597
149.199233	4792.423070	24.984615
149.618669	4810.352264	24.989632
149.499310	4821.676922	24.994650
149.882556	4814.474106	24.999667
149.475567	4837.149823	25.004685
149.881009	4838.588964	25.009703
150.137949	4853.472308	25.014720
150.447559	4863.953728	25.019738
150.730834	4865.089936	25.024755
150.654252	4847.956007	25.029773
150.749034	4855.270263	25.034791
151.047602	4870.301804	25.039808
151.415987	4874.862105	25.044826
151.490335	4879.206202	25.049843
151.610742	4878.467603	25.054861
151.458636	4881.079362	25.059879
152.028927	4895.626720	25.064896
151.940279	4899.844692	25.069914
152.048011	4900.291724	25.074931
152.394416	4908.400122	25.079949
152.586612	4916.557784	25.084967
152.608397	4930.010063	25.089984
152.938679	4924.816627	25.095002
153.113572	4927.806757	25.100019
152.804685	4934.966097	25.105037
153.149468	4930.711019	25.110055
153.443106	4946.201074	25.115072
153.477592	4945.157049	25.120090
154.032213	4943.154556	25.125107
153.966428	4950.402312	25.130125
153.937085	4935.662992	25.135143
154.063195	4956.238898	25.140160
154.026193	4970.075976	25.145178
154.485329	4965.938812	25.150195
154.277981	4972.533139	25.155213
154.106653	4975.735002	25.160231
154.702107	4994.075718	25.165248
155.167128	5003.406174	25.170266
155.239750	4996.021227	25.175283
155.107068	5019.443574	25.180301
155.183727	5018.954827	25.185319
155.365748	5032.499023	25.190336
155.398332	5036.543485	25.195354
155.888175	5048.199559	25.200371
155.822063	5059.307749	25.205389
155.920795	5058.727184	25.210407
156.094180	5071.152213	25.215424
156.327323	5078.688064	25.220442
156.765270	5089.995564	25.225459
156.681333	5101.895671	25.230477
156.713511	5101.833656	25.235495
157.194336	5116.136291	25.240512
157.344555	5121.645995	25.245530
157.787457	5121.977722	25.250547
158.488205	5109.820213	25.255565
159.021113	5093.531787	25.260583
159.188134	5093.243608	25.265600
158.932531	5096.253442	25.270618
159.207594	5082.830201	25.275635
159.132988	5094.672034	25.280653
159.558432	5087.371003	25.285671
159.287084	5085.512873	25.290688
159.566944	5083.455292	25.295706
159.741132	5080.167364	25.300723
159.089388	5082.266682	25.305741
159.479741	5089.759123	25.310759
159.528499	5083.271135	25.315776
159.275182	5092.186345	25.320794
159.539750	5108.735322	25.325811
159.734813	5110.961635	25.330829
159.949096	5126.287436	25.335847
159.993661	5130.964504	25.340864
160.263833	5147.856699	25.345882
160.740237	5168.665548	25.350899
160.325597	5174.092762	25.355917
160.348435	5167.050083	25.360935
160.686501	5172.833578	25.365952
160.949656	5197.772764	25.370970
161.001486	5203.319907	25.375987
161.338718	5216.761164	25.381005
161.318347	5230.056092	25.386023
161.837481	5237.266556	25.391040
161.687170	5251.456076	25.396058
161.931572	5256.376678	25.401075
161.644592	5273.374671	25.406093
162.398856	5276.969084	25.411111
162.733395	5289.599597	25.416128
162.450621	5300.962622	25.421146
162.997762	5310.978036	25.426163
162.987534	5321.307501	25.431181
163.170901	5309.934310	25.436199
163.276405	5323.405411	25.441216
163.483409	5339.610033	25.446234
164.170868	5334.395594	25.451251
164.038683	5337.780816	25.456269
163.925697	5351.740491	25.461287
164.453358	5357.952221	25.466304
164.617899	5368.409171	25.471322
164.871358	5362.921391	25.476339
164.864340	5374.317285	25.481357
165.058940	5381.969741	25.486375
165.333678	5384.612968	25.491392
165.656789	5388.031479	25.496410
165.799581	5387.664999	25.501427
165.885602	5381.079564	25.506445
165.835428	5394.309808	25.511463
166.064534	5399.677898	25.516480
166.120032	5402.169027	25.521498
166.074362	5408.744653	25.526515
166.306372	5424.345720	25.531533
166.187853	5435.253969	25.536551
166.601994	5446.742164	25.541568
166.848327	5462.571460	25.546586
167.192495	5456.602363	25.551603
166.895240	5470.180470	25.556621
167.200666	5479.460262	25.561639
167.823759	5484.312498	25.566656
167.871408	5496.940473	25.571674
168.411465	5500.625099	25.576691
168.576351	5503.983040	25.581709
168.547942	5507.686728	25.586727
168.809215	5509.037891	25.591744
168.596698	5509.471669	25.596762
168.986075	5522.592538	25.601779
169.434691	5532.295135	25.606797
169.482617	5524.696019	25.611815
169.585504	5527.795311	25.616832
169.506567	5526.049222	25.621850
169.879639	5538.632874	25.626867
169.898923	5545.331011	25.631885
170.092774	5551.070793	25.636903
170.337240	5556.528078	25.641920
170.422354	5572.076385	25.646938
170.509710	5575.013963	25.651955
170.931815	5568.025759	25.656973
171.251244	5575.406339	25.661991
171.244591	5587.140060	25.667008
171.566080	5591.685749	25.672026
171.724968	5584.372360	25.677044
171.722167	5589.258938	25.682061
171.718081	5592.864161	25.687079
171.844700	5602.184480	25.692096
172.071072	5616.672329	25.697114
172.057884	5619.234156	25.702132
172.011329	5638.054265	25.707149
171.978477	5644.656390	25.712167
172.470741	5662.679255	25.717184
172.703338	5675.411135	25.722202
172.689607	5684.191480	25.727220
173.377216	5691.577917	25.732237
173.272926	5696.477168	25.737255
173.358830	5701.681406	25.742272
173.260514	5718.158016	25.747290
173.785483	5722.747816	25.752308
174.172308	5749.975957	25.757325
173.994877	5754.226887	25.762343
174.279796	5751.931703	25.767360
174.256528	5775.293795	25.772378
174.588111	5769.500168	25.777396
175.060089	5773.571083	25.782413
175.193377	5787.735806	25.787431
175.250886	5795.621271	25.792448
175.544545	5803.012269	25.797466
175.571347	5799.380994	25.802484
175.852011	5811.802454	25.807501
175.907436	5823.214160	25.812519
176.130580	5821.070631	25.817536
176.075184	5838.538149	25.822554
176.413021	5845.906503	25.827572
176.582156	5839.923498	25.832589
176.634946	5856.392491	25.837607
176.887662	5865.683843	25.842624
176.953055	5873.842738	25.847642
176.915318	5892.563883	25.852660
177.330527	5898.114639	25.857677
177.841450	5912.640493	25.862695
178.222143	5913.651122	25.867712
178.000024	5920.648979	25.872730
178.265171	5927.113269	25.877748
178.772073	5954.177817	25.882765
178.976758	5950.458842	25.887783
179.123723	5945.404140	25.892800
178.799385	5952.585224	25.897818
179.558386	5964.379910	25.902836
179.430928	5971.978587	25.907853
179.296266	5976.017731	25.912871
179.630748	5980.482579	25.917888
179.891275	5991.272172	25.922906
180.117992	5993.541014	25.927924
180.162116	6005.099798	25.932941
180.195622	6013.298442	25.937959
180.302164	6026.637324	25.942976
180.406893	6044.032760	25.947994
180.904053	6050.596707	25.953012
181.523015	6060.591885	25.958029
181.420228	6070.604739	25.963047
181.684603	6072.204837	25.968064
182.064356	6081.315534	25.973082
182.312288	6089.281961	25.978100
182.581285	6091.907246	25.983117
182.912151	6083.297917	25.988135
182.794306	6076.156838	25.993152
182.927234	6092.765086	25.998170
182.703182	6098.270224	26.003188
182.954601	6096.699925	26.008205
183.228574	6107.553782	26.013223
183.193607	6125.012080	26.018240
183.394193	6133.352068	26.023258
183.414469	6147.692497	26.028276
183.930529	6160.535260	26.033293
183.780554	6168.030199	26.038311
184.314130	6184.554057	26.043328
184.334309	6199.090254	26.048346
184.526472	6194.334642	26.053364
184.859103	6207.654240	26.058381
184.917195	6213.096546	26.063399
184.848280	6224.871937	26.068416
185.293970	6243.713890	26.073434
185.728011	6250.136217	26.078452
186.015062	6251.312964	26.083469
186.138752	6269.718951	26.088487
186.342896	6268.809427	26.093504
186.495751	6277.652508	26.098522
186.584969	6285.438548	26.103540
187.143047	6289.335185	26.108557
187.214807	6298.456062	26.113575
187.055035	6297.521121	26.118592
187.478613	6294.292005	26.123610
187.230565	6302.007450	26.128628
187.684747	6306.870424	26.133645
187.784749	6319.610771	26.138663
187.678356	6318.004617	26.143680
188.028247	6323.338393	26.148698
188.022665	6342.342250	26.153716
187.917565	6344.138789	26.158733
188.570393	6368.583290	26.163751
188.700158	6375.270844	26.168768
188.966313	6387.448735	26.173786
189.414053	6396.435364	26.178804
189.498623	6392.558227	26.183821
189.429485	6408.200709	26.188839
189.814682	6413.298576	26.193856
189.950773	6426.371145	26.198874
189.770090	6448.858949	26.203892
190.261031	6440.963198	26.208909
190.241996	6464.840053	26.213927
190.441346	6467.754026	26.218944
191.212626	6479.256720	26.223962
191.461014	6487.191684	26.228980
191.561414	6485.022994	26.233997
191.632715	6488.436724	26.239015
191.852155	6503.576638	26.244032
192.263103	6506.164100	26.249050
192.434770	6515.679902	26.254068
192.919683	6506.162514	26.259085
192.829541	6520.602502	26.264103
193.093404	6531.388738	26.269120
193.361421	6533.651219	26.274138
193.419820	6531.425929	26.279156
193.602204	6526.996894	26.284173
193.414835	6551.941785	26.289191
193.544233	6557.660353	26.294208
194.200479	6555.843899	26.299226
193.786362	6581.894258	26.304244
193.954326	6580.210643	26.309261
194.112913	6596.423921	26.314279
194.662005	6613.204604	26.319296
194.838179	6628.897470	26.324314
194.883640	6643.565824	26.329332
195.282149	6644.308557	26.334349
195.266487	6670.637934	26.339367
195.390005	6673.999375	26.344384
195.762912	6676.324462	26.349402
195.843359	6696.527478	26.354420
196.089801	6692.110528	26.359437
196.398408	6702.826765	26.364455
196.716508	6724.075573	26.369472
196.651733	6724.997767	26.374490
197.349407	6736.815131	26.379508
197.700591	6739.812838	26.384525
197.847023	6752.751448	26.389543
197.631599	6747.809766	26.394560
198.101459	6758.586163	26.399578
198.004193	6774.009207	26.404596
198.458659	6771.940040	26.409613
198.654645	6782.882204	26.414631
198.595982	6792.755999	26.419648
198.917056	6793.946426	26.424666
198.570422	6796.882320	26.429684
198.815997	6803.832953	26.434701
198.942656	6831.077959	26.439719
199.159209	6844.308764	26.444736
199.628682	6850.091278	26.449754
199.858553	6871.982190	26.454772
199.984730	6874.096332	26.459789
200.101115	6880.609375	26.464807
200.379598	6888.912327	26.469824
200.845146	6895.064809	26.474842
200.695429	6906.297626	26.479860
200.985179	6919.662301	26.484877
200.993420	6926.848808	26.489895
201.227278	6946.330568	26.494912
201.882707	6944.703612	26.499930
201.824450	6963.602670	26.504948
201.831621	6972.714998	26.509965
201.889427	6989.436773	26.514983
202.084033	6999.081841	26.520000
202.614454	7013.678145	26.525018
202.586150	7027.859517	26.530036
202.828316	7030.729033	26.535053
203.297273	7049.969110	26.540071
203.535170	7049.827709	26.545088
204.026261	7056.033091	26.550106
204.302967	7055.282699	26.555124
204.970070	7063.913513	26.560141
205.109063	7055.803965	26.565159
205.388309	7056.180155	26.570176
205.857480	7050.617250	26.575194
205.880692	7060.592087	26.580212
206.273509	7046.239916	26.585229
206.063091	7057.365474	26.590247
206.072059	7057.537513	26.595264
206.166264	7052.159257	26.600282
206.530586	7065.064164	26.605300
206.738943	7063.260572	26.610317
206.744633	7071.486119	26.615335
206.863289	7071.966231	26.620352
207.310620	7088.488554	26.625370
207.069524	7098.719224	26.630388
207.215825	7096.960014	26.635405
207.363554	7115.663006	26.640423
207.626226	7133.148533	26.645440
207.974784	7135.875229	26.650458
207.671414	7155.996451	26.655476
207.899264	7159.490109	26.660493
208.210104	7176.046388	26.665511
208.242897	7187.822346	26.670528
208.718330	7195.848543	26.675546
208.882442	7210.236861	26.680564
209.366248	7217.778770	26.685581
209.313246	7229.587054	26.690599
209.723994	7252.971852	26.695616
209.947160	7249.366542	26.700634
210.132454	7270.807130	26.705652
210.130171	7281.502658	26.710669
210.534155	7282.695995	26.715687
210.613309	7310.634144	26.720704
210.914520	7315.868458	26.725722
211.072772	7331.713088	26.730740
211.233734	7341.496162	26.735757
211.665020	7356.758486	26.740775
211.577044	7366.637153	26.745792
212.023190	7384.482648	26.750810
211.913486	7392.252776	26.755828
212.081376	7409.358716	26.760845
212.463227	7421.885479	26.765863
212.393411	7450.633091	26.770880
212.935689	7443.073018	26.775898
212.932221	7472.182845	26.780916
213.552817	7475.915320	26.785933
213.662213	7489.576825	26.790951
213.877482	7500.705828	26.795968
214.295889	7496.814366	26.800986
214.123886	7513.023100	26.806004
214.241559	7530.667326	26.811021
214.652715	7523.525402	26.816039
214.865645	7559.227965	26.821056
215.287117	7555.414936	26.826074
215.386812	7574.362640	26.831092
215.257134	7579.935606	26.836109
215.866147	7582.249307	26.841127
215.751360	7601.893378	26.846144
216.080312	7606.640452	26.851162
216.146793	7631.263166	26.856180
216.311301	7639.098041	26.861197
216.671315	7657.879026	26.866215
217.105850	7667.736488	26.871232
216.974344	7674.395742	26.876250
217.301277	7688.320276	26.881268
217.829757	7702.822726	26.886285
217.584360	7699.808011	26.891303
217.865239	7728.188923	26.896320
218.438781	7738.993954	26.901338
218.841968	7748.449097	26.906356
219.419910	7750.890778	26.911373
219.838367	7757.192945	26.916391
219.563867	7757.828993	26.921408
219.684508	7776.391656	26.926426
219.748449	7784.276977	26.931444
219.979193	7794.418788	26.936461
220.256653	7806.753710	26.941479
220.567839	7809.397933	26.946496
220.875377	7816.771803	26.951514
221.324101	7826.295663	26.956532
221.515907	7825.110176	26.961549
221.381429	7840.274725	26.966567
221.838796	7854.977783	26.971584
222.053609	7845.217634	26.976602
221.898808	7864.018999	26.981620
222.101820	7870.585204	26.986637
222.464321	7889.549141	26.991655
222.753346	7905.288669	26.996672
222.754283	7906.121768	27.001690
223.245113	7921.293211	27.006708
223.462685	7928.908433	27.011725
223.742561	7952.466031	27.016743
223.720011	7963.262976	27.021760
224.043967	7972.468544	27.026778
224.493134	7986.683656	27.031796
224.865644	7984.570292	27.036813
225.035451	7987.811118	27.041831
225.293835	8003.656523	27.046848
225.345088	8000.554533	27.051866
225.653450	8018.491550	27.056884
225.653891	8028.445201	27.061901
225.764654	8035.751929	27.066919
225.884931	8055.691368	27.071936
226.361988	8061.416263	27.076954
226.598052	8081.899645	27.081972
226.459928	8086.378608	27.086989
226.611865	8094.345071	27.092007
227.253710	8119.207186	27.097024
227.221138	8117.958747	27.102042
227.544591	8137.165793	27.107060
227.926138	8145.229123	27.112077
228.490219	8155.979048	27.117095
228.735891	8163.883593	27.122112
229.175172	8153.396954	27.127130
229.525494	8159.094255	27.132148
229.391166	8176.301629	27.137165
229.892183	8175.412091	27.142183
229.921215	8184.237487	27.147200
230.046037	8173.698770	27.152218
230.204852	8174.974536	27.157236
230.087746	8186.405103	27.162253
230.070675	8188.595368	27.167271
230.633782	8209.435228	27.172288
230.576017	8220.490366	27.177306
230.562052	8228.021793	27.182324
230.908696	8238.941370	27.187341
231.228066	8253.918792	27.192359
231.612268	8268.668300	27.197376
231.715838	8278.173520	27.202394
232.144191	8294.475737	27.207412
232.115543	8302.277826	27.212429
232.849795	8321.004383	27.217447
232.797997	8340.020658	27.222464
232.765938	8351.220252	27.227482
233.363615	8361.772489	27.232500
233.524256	8384.430510	27.237517
233.913458	8385.124257	27.242535
233.975169	8399.406324	27.247552
234.421764	8412.182561	27.252570
234.105378	8414.823552	27.257588
234.413280	8437.559737	27.262605
234.551900	8446.286114	27.267623
234.951812	8459.366413	27.272640
235.169855	8476.976978	27.277658
235.100781	8497.596725	27.282676
235.529992	8514.337832	27.287693
236.071096	8524.876871	27.292711
236.169171	8544.949735	27.297728
236.631189	8552.991246	27.302746
237.245254	8570.155083	27.307764
237.078691	8585.928238	27.312781
237.283345	8591.597839	27.317799
237.578275	8609.054492	27.322816
237.667311	8625.810776	27.327834
238.008208	8631.778043	27.332852
238.118175	8644.114347	27.337869
238.752880	8652.315283	27.342887
238.951326	8666.339489	27.347904
239.382345	8681.621898	27.352922
239.281011	8686.957161	27.357940
239.578801	8700.410280	27.362957
239.890004	8708.434297	27.367975
240.093082	8718.331516	27.372992
240.545740	8732.489834	27.378010
240.799855	8740.658507	27.383028
240.667025	8758.705974	27.388045
241.106279	8763.303579	27.393063
241.469176	8773.848407	27.398080
242.011146	8776.055890	27.403098
242.158329	8782.002851	27.408116
242.177956	8792.095996	27.413133
242.595960	8804.327622	27.418151
242.531198	8822.522409	27.423168
242.820057	8824.965044	27.428186
242.394616	8841.580624	27.433204
243.002967	8855.020234	27.438221
243.385962	8863.459351	27.443239
243.116805	8880.729413	27.448256
243.396996	8893.235123	27.453274
243.909335	8908.501903	27.458292
244.030143	8916.921878	27.463309
244.586834	8933.135223	27.468327
244.724346	8948.586676	27.473344
244.837426	8957.913967	27.478362
245.461420	8967.685804	27.483380
245.217836	8972.313999	27.488397
245.826126	8998.517991	27.493415
245.943679	9009.170606	27.498432
245.891229	9017.718630	27.503450
246.382860	9036.973044	27.508468
246.558466	9054.972780	27.513485
246.930293	9062.015114	27.518503
247.440155	9069.417974	27.523520
247.934790	9067.910591	27.528538
248.300805	9070.963205	27.533556
248.242127	9078.056782	27.538573
248.628084	9085.943040	27.543591
248.476582	9100.887116	27.548608
249.007667	9104.365508	27.553626
249.210204	9111.727832	27.558644
249.476716	9133.852517	27.563661
249.854737	9136.432856	27.568679
250.194328	9141.418617	27.573696
250.239563	9146.087133	27.578714
250.353866	9152.547635	27.583732
250.388101	9163.810014	27.588749
250.436759	9188.162906	27.593767
250.631456	9203.293110	27.598784
250.989617	9225.915098	27.603802
251.587037	9227.681472	27.608820
251.151391	9248.835858	27.613837
251.478906	9262.572063	27.618855
252.221661	9280.493193	27.623872
251.823055	9293.890990	27.628890
252.814289	9309.964399	27.633908
252.938027	9329.225880	27.638925
253.724918	9331.632090	27.643943
253.633795	9339.425400	27.648960
253.521436	9355.241285	27.653978
254.278049	9359.584414	27.658996
254.207888	9389.212796	27.664013
254.609044	9394.113268	27.669031
255.263006	9398.788108	27.674048
254.875885	9415.091985	27.679066
255.565530	9429.709624	27.684084
255.893067	9437.428324	27.689101
255.949019	9455.968018	27.694119
256.154565	9474.446554	27.699136
256.144522	9478.624920	27.704154
256.893405	9481.545380	27.709172
256.672965	9496.986718	27.714189
257.004682	9511.110790	27.719207
257.265256	9528.658905	27.724224
257.760322	9538.751054	27.729242
257.954996	9560.360176	27.734260
258.189801	9579.595153	27.739277
258.349895	9586.061306	27.744295
258.411020	9592.334492	27.749312
258.833499	9611.521340	27.754330
259.238416	9627.749453	27.759348
259.252392	9649.364711	27.764365
259.534569	9657.946177	27.769383
260.142183	9672.545207	27.774400
260.143221	9689.653980	27.779418
260.870174	9699.877449	27.784436
260.995657	9715.659770	27.789453
261.085726	9717.751446	27.794471
261.532377	9727.336603	27.799488
261.417085	9736.813502	27.804506
262.164357	9751.343493	27.809524
261.990224	9754.824456	27.814541
262.189351	9776.098467	27.819559
262.571391	9783.530987	27.824576
262.922721	9803.171128	27.829594
263.009908	9814.239380	27.834612
263.022322	9821.647372	27.839629
263.457314	9840.223156	27.844647
263.752630	9847.148253	27.849664
263.909774	9869.796008	27.854682
264.127294	9877.396257	27.859700
264.433330	9901.826834	27.864717
264.351883	9903.525316	27.869735
264.910230	9919.758213	27.874752
265.462670	9943.743195	27.879770
265.401184	9945.744829	27.884788
265.926129	9967.805017	27.889805
265.883704	9974.264947	27.894823
266.417204	9989.273585	27.899840
266.542100	10006.025535	27.904858
267.239998	10020.913885	27.909876
267.296240	10030.323183	27.914893
267.700854	10053.185218	27.919911
268.058241	10065.010352	27.924928
267.916191	10074.715758	27.929946
268.404874	10088.856878	27.934964
268.671234	10101.927560	27.939981
268.703198	10108.110741	27.944999
268.897909	10115.976696	27.950016
268.805430	10136.952371	27.955034
269.376578	10154.572704	27.960052
269.710941	10183.779437	27.965069
269.918297	10203.161413	27.970087
270.359240	10222.065016	27.975104
270.228448	10231.718233	27.980122
271.174127	10235.744821	27.985140
271.653068	10260.827780	27.990157
271.412187	10271.325382	27.995175
272.218274	10276.794517	28.000192
272.327413	10299.816521	28.005210
272.653748	10326.902988	28.010228
273.047345	10331.378644	28.015245
273.170838	10332.328538	28.020263
273.403448	10357.061622	28.025280
273.070474	10367.497838	28.030298
273.735970	10383.900746	28.035316
274.031341	10405.084715	28.040333
274.125601	10420.206289	28.045351
274.423519	10438.437757	28.050368
274.747443	10454.518177	28.055386
274.795550	10466.293838	28.060404
275.045129	10493.897679	28.065421
275.313416	10511.050848	28.070439
275.650372	10537.232954	28.075456
275.960811	10560.814373	28.080474
275.948469	10565.097536	28.085492
276.359167	10590.381007	28.090509
276.741768	10609.802429	28.095527
277.681640	10627.005862	28.100544
277.606024	10645.062038	28.105562
277.869136	10653.526952	28.110580
278.238718	10663.257205	28.115597
278.947621	10664.996894	28.120615
279.341439	10681.470778	28.125632
279.216222	10695.155388	28.130650
279.630606	10711.370345	28.135668
279.961630	10715.407482	28.140685
280.190173	10719.618446	28.145703
280.467155	10737.799791	28.150720
280.332861	10748.451567	28.155738
280.780203	10770.227990	28.160756
281.063381	10772.595993	28.165773
281.265150	10786.914926	28.170791
281.670377	10792.778155	28.175808
281.696151	10815.412780	28.180826
281.998581	10822.289773	28.185844
282.492815	10836.746343	28.190861
282.748161	10853.052490	28.195879
282.937527	10864.149662	28.200896
283.255017	10882.640586	28.205914
283.402019	10895.648314	28.210932
283.425026	10909.695214	28.215949
283.719507	10923.917725	28.220967
284.086471	10942.331542	28.225984
284.222323	10962.445341	28.231002
284.657034	10981.470669	28.236020
284.669660	10990.599913	28.241037
285.009511	11011.240877	28.246055
285.818535	11023.580440	28.251072
285.977262	11046.096763	28.256090
286.665630	11048.733255	28.261108
286.828037	11057.687653	28.266125
287.126877	11073.046292	28.271143
287.671806	11082.440032	28.276160
287.677054	11093.272358	28.281178
287.856903	11105.649937	28.286196
288.163522	11109.305746	28.291213
288.179703	11138.503519	28.296231
288.550545	11148.751659	28.301248
288.865988	11165.579182	28.306266
289.352649	11186.229058	28.311284
289.694340	11196.573330	28.316301
289.907155	11223.489323	28.321319
290.302057	11222.003617	28.326336
290.577810	11240.747680	28.331354
290.694262	11248.954679	28.336372
291.039222	11271.811710	28.341389
291.442249	11283.614726	28.346407
291.841232	11297.729685	28.351424
291.812736	11310.348232	28.356442
292.112762	11327.847696	28.361460
292.480660	11338.219542	28.366477
292.800570	11366.243146	28.371495
293.174647	11370.895758	28.376512
293.622343	11393.310676	28.381530
293.881836	11402.853215	28.386548
293.785233	11422.425869	28.391565
293.825584	11425.112782	28.396583
294.410410	11445.277188	28.401600
294.520583	11472.468438	28.406618
294.939221	11489.659093	28.411636
294.992184	11506.287813	28.416653
295.341679	11535.074350	28.421671
296.106669	11542.902646	28.426688
295.767027	11563.814200	28.431706
296.093787	11580.719275	28.436724
296.697221	11600.063141	28.441741
297.200591	11627.572309	28.446759
297.654241	11635.960643	28.451776
297.944471	11653.165125	28.456794
297.817048	11665.032019	28.461812
298.338558	11681.947914	28.466829
298.532799	11697.452812	28.471847
298.851049	11713.408897	28.476864
298.893974	11733.421161	28.481882
299.205175	11754.061090	28.486900
300.502461	11761.844500	28.491917
300.669147	11768.900857	28.496935
301.166334	11770.487319	28.501952
301.268511	11790.777761	28.506970
301.473373	11799.170167	28.511988
302.214775	11798.366196	28.517005
302.041768	11807.227922	28.522023
301.865777	11812.856727	28.527040
301.921367	11834.294366	28.532058
302.297467	11838.574182	28.537076
302.928640	11852.776559	28.542093
302.872718	11874.016886	28.547111
303.339884	11889.643648	28.552128
303.377549	11908.835937	28.557146
303.737885	11925.818194	28.562164
304.204674	11945.840479	28.567181
304.177093	11955.557456	28.572199
304.709991	11972.847599	28.577216
304.979557	11998.016013	28.582234
305.332085	12015.852130	28.587252
305.906061	12033.817985	28.592269
305.902974	12051.690553	28.597287
306.412032	12070.654894	28.602304
306.262818	12094.846610	28.607322
306.754801	12114.148365	28.612340
307.589351	12131.483265	28.617357
307.497751	12155.590305	28.622375
307.800388	12171.340805	28.627392
308.004329	12196.143938	28.632410
307.891223	12219.815493	28.637428
308.244531	12241.453544	28.642445
308.463367	12264.290372	28.647463
308.893263	12291.988784	28.652480
308.847301	12311.071353	28.657498
309.316662	12333.468235	28.662516
309.934647	12370.026393	28.667533
310.197352	12392.240795	28.672551
310.487100	12414.943615	28.677568
311.135042	12429.052245	28.682586
311.810527	12447.365830	28.687604
312.297843	12464.259336	28.692621
312.569525	12482.436885	28.697639
312.992663	12502.482349	28.702656
313.358936	12512.548800	28.707674
313.130038	12528.511818	28.712692
313.682789	12544.031071	28.717709
314.014117	12574.764035	28.722727
314.009261	12579.908554	28.727744
314.392039	12603.844425	28.732762
314.647113	12620.998428	28.737780
315.429625	12645.737342	28.742797
315.257941	12669.267008	28.747815
316.060591	12681.772868	28.752832
316.404435	12697.113201	28.757850
316.817998	12708.931266	28.762868
317.222058	12714.713182	28.767885
317.634204	12733.219617	28.772903
318.143057	12748.164844	28.777920
318.164247	12741.883722	28.782938
318.221184	12766.846277	28.787956
318.572579	12776.296264	28.792973
318.720934	12792.649176	28.797991
319.092386	12812.715649	28.803008
319.293331	12833.904436	28.808026
319.713215	12846.362633	28.813044
320.350141	12847.892700	28.818061
320.574000	12870.344232	28.823079
320.913727	12894.792421	28.828096
321.560316	12897.552526	28.833114
321.863177	12915.473016	28.838132
322.306080	12906.517849	28.843149
322.205287	12919.246622	28.848167
322.395091	12932.545933	28.853184
322.571238	12934.416155	28.858202
322.595232	12969.403795	28.863220
322.845135	12969.311018	28.868237
323.099234	12991.435891	28.873255
323.445823	13022.290365	28.878272
323.802406	13032.942799	28.883290
324.014428	13057.673179	28.888308
324.296186	13069.433046	28.893325
324.589077	13099.380238	28.898343
324.892253	13117.964015	28.903360
325.377752	13140.700392	28.908378
325.413725	13165.429901	28.913396
325.990543	13187.255292	28.918413
326.211486	13209.988730	28.923431
326.564770	13233.885783	28.928448
326.696161	13261.919459	28.933466
326.807270	13285.566917	28.938484
327.508923	13304.742517	28.943501
328.338017	13324.826708	28.948519
329.285506	13325.174795	28.953536
329.846069	13340.576649	28.958554
330.085512	13353.075904	28.963572
330.470994	13359.896692	28.968589
330.545305	13373.880604	28.973607
330.314152	13388.748918	28.978624
330.833172	13403.977293	28.983642
331.152545	13416.729408	28.988660
331.257339	13436.746481	28.993677
331.393927	13456.104944	28.998695
331.949536	13473.295039	29.003712
332.071122	13493.975872	29.008730
332.310433	13529.647868	29.013748
332.589249	13543.249541	29.018765
332.824837	13568.816922	29.023783
333.286324	13586.321775	29.028800
334.308394	13604.304636	29.033818
334.705026	13617.098543	29.038836
334.944237	13626.863267	29.043853
335.367001	13641.124709	29.048871
335.793914	13664.426631	29.053888
336.041432	13669.781631	29.058906
336.173222	13694.891655	29.063924
336.622719	13705.138422	29.068941
337.053442	13724.252418	29.073959
336.982760	13749.097190	29.078976
337.651432	13760.244613	29.083994
337.177425	13787.094355	29.089012
338.248549	13800.771815	29.094029
338.756812	13822.788617	29.099047
338.657522	13835.063028	29.104064
339.396235	13847.421724	29.109082
339.422496	13876.385324	29.114100
340.306561	13889.810913	29.119117
340.753896	13907.611957	29.124135
340.325272	13920.957715	29.129152
340.969004	13924.855286	29.134170
340.971850	13950.772055	29.139188
341.292827	13980.043624	29.144205
341.468325	14000.801882	29.149223
341.749437	14022.254265	29.154240
342.330595	14044.278925	29.159258
342.696182	14069.747795	29.164276
343.233274	14073.519890	29.169293
343.316135	14098.028574	29.174311
343.489068	14118.569459	29.179328
344.000495	14128.721550	29.184346
344.225026	14160.806396	29.189364
344.726966	14174.310626	29.194381
344.912327	14191.404276	29.199399
345.007449	14223.717803	29.204416
345.557645	14229.123739	29.209434
345.739608	14266.072412	29.214452
345.991825	14279.182946	29.219469
346.630035	14305.509726	29.224487
346.420011	14331.169616	29.229504
347.408108	14347.456300	29.234522
347.580090	14381.896117	29.239540
347.762160	14409.001454	29.244557
348.415670	14426.148753	29.249575
348.851083	14445.357489	29.254592
348.961686	14468.119089	29.259610
349.352012	14488.449679	29.264628
349.694074	14513.044867	29.269645
350.068256	14536.981368	29.274663
350.222131	14556.047720	29.279680
350.983793	14572.480383	29.284698
351.285371	14600.767453	29.289716
351.493395	14617.719003	29.294733
351.929556	14634.376088	29.299751
352.372873	14659.843123	29.304768
352.932796	14679.661170	29.309786
352.678735	14708.394926	29.314804
353.385525	14731.834600	29.319821
353.781627	14757.757566	29.324839
353.918694	14784.971503	29.329856
354.421014	14806.330331	29.334874
354.699913	14828.611394	29.339892
354.946195	14849.975392	29.344909
355.570170	14874.220822	29.349927
355.687741	14902.751740	29.354944
356.477914	14920.007694	29.359962
356.694459	14940.479515	29.364980
357.005957	14962.221936	29.369997
357.365316	14982.864215	29.375015
357.454014	15008.986971	29.380032
358.056812	15025.937430	29.385050
358.359542	15059.439099	29.390068
358.705682	15083.832268	29.395085
359.098423	15111.148985	29.400103
359.307771	15132.749595	29.405120
359.814275	15155.617765	29.410138
360.118317	15185.860225	29.415156
360.300771	15206.659773	29.420173
360.968005	15227.273336	29.425191
361.017636	15260.457886	29.430208
361.243646	15281.493915	29.435226
361.587790	15313.530500	29.440244
362.228185	15342.874450	29.445261
362.778385	15368.711094	29.450279
362.798550	15399.171788	29.455296
363.279516	15419.400833	29.460314
363.661404	15445.320631	29.465332
364.294853	15467.806218	29.470349
364.754171	15483.595091	29.475367
365.088819	15497.814801	29.480384
365.607038	15515.483147	29.485402
366.210644	15537.506045	29.490420
366.629745	15553.026471	29.495437
366.730378	15576.912119	29.500455
366.712866	15595.807225	29.505472
367.525863	15604.545642	29.510490
367.590085	15641.736388	29.515508
367.973000	15655.774998	29.520525
368.389655	15666.132163	29.525543
368.668028	15686.724648	29.530560
369.144823	15702.694161	29.535578
369.493007	15726.039293	29.540596
369.852448	15737.362357	29.545613
370.037445	15760.372895	29.550631
370.360439	15789.141609	29.555648
370.526144	15809.205386	29.560666
371.045882	15831.573299	29.565684
371.376672	15852.246234	29.570701
371.536606	15873.789052	29.575719
371.787156	15908.074112	29.580736
372.270990	15926.253518	29.585754
372.955360	15947.793732	29.590772
373.382026	15974.335778	29.595789
373.956366	16007.196747	29.600807
373.786710	16023.788290	29.605824
374.450198	16044.927600	29.610842
374.848031	16061.914050	29.615860
375.750542	16068.115253	29.620877
376.809573	16067.024807	29.625895
377.445665	16083.241454	29.630912
377.832535	16091.976954	29.635930
378.101391	16094.805822	29.640948
378.188317	16105.653565	29.645965
378.569900	16117.046049	29.650983
378.449405	16139.577163	29.656000
378.675390	16147.860828	29.661018
378.764649	16167.103083	29.666036
379.153276	16186.248217	29.671053
379.757691	16202.030888	29.676071
379.816695	16235.323054	29.681088
380.143242	16252.737672	29.686106
380.605584	16278.188116	29.691124
381.059132	16310.095639	29.696141
381.429423	16334.019210	29.701159
381.496049	16361.063173	29.706176
381.818515	16381.507415	29.711194
382.445122	16402.596013	29.716212
382.546642	16439.286637	29.721229
383.386034	16462.818342	29.726247
383.296142	16489.226751	29.731264
384.068794	16517.778113	29.736282
384.307308	16539.555800	29.741300
384.722370	16568.589291	29.746317
385.165402	16593.499915	29.751335
385.367830	16618.296425	29.756352
385.441966	16650.020384	29.761370
385.975089	16676.963741	29.766388
386.465301	16713.935486	29.771405
386.682312	16736.973797	29.776423
386.978084	16776.780615	29.781440
387.213616	16800.463597	29.786458
387.613344	16825.062260	29.791476
388.412876	16859.415160	29.796493
389.215571	16882.093997	29.801511
389.627127	16911.096967	29.806528
390.045202	16932.843987	29.811546
390.608287	16963.481637	29.816564
390.728948	16979.457124	29.821581
391.151917	17003.840782	29.826599
391.439678	17030.993392	29.831616
392.142299	17055.785240	29.836634
392.326594	17080.461989	29.841652
392.387248	17108.967152	29.846669
392.899945	17126.697859	29.851687
393.427642	17146.763532	29.856704
393.864664	17170.245042	29.861722
394.170390	17207.726549	29.866740
394.496871	17222.113054	29.871757
394.604835	17251.069045	29.876775
394.587248	17276.750295	29.881792
395.290007	17293.368197	29.886810
396.268748	17320.318887	29.891828
396.195015	17345.446752	29.896845
396.592099	17369.165296	29.901863
396.690455	17396.783785	29.906880
397.230263	17415.347549	29.911898
397.726032	17445.547934	29.916916
398.339646	17472.603059	29.921933
398.889624	17489.036452	29.926951
399.492110	17511.804056	29.931968
399.546499	17537.212287	29.936986
400.257540	17562.142455	29.942004
400.113870	17593.526007	29.947021
400.752583	17617.507303	29.952039
401.273544	17647.236613	29.957056
401.623247	17677.302172	29.962074
402.281919	17688.999897	29.967092
402.902351	17709.301248	29.972109
403.462439	17723.099008	29.977127
404.085773	17751.953407	29.982144
404.145594	17756.864992	29.987162
404.754309	17778.343236	29.992180
404.745700	17801.699060	29.997197
405.514590	17808.831317	30.002215
405.692582	17834.362833	30.007232
405.790413	17855.762768	30.012250
406.339548	17877.566260	30.017268
406.922973	17906.382883	30.022285
407.212617	17921.896955	30.027303
407.390589	17949.829178	30.032320
407.459936	17980.873809	30.037338
408.340108	18007.869237	30.042356
408.489923	18041.794746	30.047373
409.159663	18060.098848	30.052391
409.499262	18088.132455	30.057408
409.524030	18111.761417	30.062426
410.123475	18134.896635	30.067444
410.096227	18177.757354	30.072461
410.425026	18195.274459	30.077479
411.015748	18232.220835	30.082496
411.761811	18261.075841	30.087514
412.659989	18281.220843	30.092532
412.754780	18320.272465	30.097549
413.425979	18348.539107	30.102567
413.590273	18380.498251	30.107584
413.954536	18394.554404	30.112602
414.465546	18424.558109	30.117620
414.840457	18450.514635	30.122637
415.430643	18474.428743	30.127655
415.694348	18498.589547	30.132672
416.358899	18524.753779	30.137690
416.606597	18550.306975	30.142708
416.975657	18576.624675	30.147725
417.209111	18608.396539	30.152743
417.792955	18628.306554	30.157760
418.223010	18654.918103	30.162778
418.900416	18671.023110	30.167796
419.554289	18697.151333	30.172813
420.230798	18722.555872	30.177831
420.578215	18731.996801	30.182848
420.798329	18749.127007	30.187866
421.252889	18768.930943	30.192884
421.350942	18797.186388	30.197901
421.948814	18800.416140	30.202919
422.220590	18829.440595	30.207936
422.062046	18848.139729	30.212954
422.886256	18865.984638	30.217972
423.254349	18896.617808	30.222989
423.520984	18912.799600	30.228007
423.707809	18936.979237	30.233024
424.146614	18967.961612	30.238042
424.723235	18992.510230	30.243060
425.335377	19010.053455	30.248077
426.560496	19016.142228	30.253095
427.248780	19033.894737	30.258112
427.575509	19056.467025	30.263130
427.868094	19057.811160	30.268148
428.018574	19077.163660	30.273165
428.015218	19099.225117	30.278183
428.587725	19114.891956	30.283200
429.011591	19145.365213	30.288218
429.302486	19166.155315	30.293236
429.324109	19186.658843	30.298253
430.005075	19203.218610	30.303271
430.217417	19237.844054	30.308288
430.634518	19261.722903	30.313306
431.100419	19287.590573	30.318324
431.567885	19329.820861	30.323341
431.831293	19367.471080	30.328359
432.559447	19383.480332	30.333376
432.483663	19421.897363	30.338394
432.542290	19452.345831	30.343412
433.144590	19499.262210	30.348429
433.514610	19526.294954	30.353447
434.349191	19557.981105	30.358464
434.596657	19603.108185	30.363482
435.236069	19624.217269	30.368500
435.918543	19666.718070	30.373517
436.483878	19683.928030	30.378535
436.938697	19714.428948	30.383552
437.380467	19746.827295	30.388570
438.088195	19763.680313	30.393588
438.505619	19792.304460	30.398605
438.902641	19819.541897	30.403623
439.456972	19843.785486	30.408640
439.764259	19867.164109	30.413658
440.480004	19893.916098	30.418676
440.603554	19912.964044	30.423693
441.271485	19936.829945	30.428711
441.577798	19971.372565	30.433728
442.024975	19997.048237	30.438746
442.798170	20024.360074	30.443764
442.781162	20052.951149	30.448781
443.532276	20075.812355	30.453799
443.960682	20098.559560	30.458816
444.181966	20131.826840	30.463834
444.622392	20155.810560	30.468852
444.941521	20173.514176	30.473869
445.283041	20207.691609	30.478887
445.674040	20232.441276	30.483904
446.039335	20265.547368	30.488922
447.109649	20285.301216	30.493940
447.462766	20325.422294	30.498957
447.940169	20353.216584	30.503975
448.237124	20377.153413	30.508992
448.186880	20410.103310	30.514010
448.801096	20427.078868	30.519028
449.419617	20469.932549	30.524045
449.248158	20501.997987	30.529063
449.701702	20531.255720	30.534080
450.335896	20566.544426	30.539098
450.593546	20603.130165	30.544116
451.586985	20640.890322	30.549133
451.773924	20658.475958	30.554151
451.935684	20678.655964	30.559168
452.052510	20725.518186	30.564186
452.719608	20746.636813	30.569204
453.002297	20784.343623	30.574221
453.887677	20822.771725	30.579239
454.115536	20852.121935	30.584256
454.287993	20896.107447	30.589274
454.953695	20926.672200	30.594292
455.113702	20965.144006	30.599309
455.918913	21000.501644	30.604327
456.676340	21033.762809	30.609344
456.994713	21074.010874	30.614362
457.710264	21104.283823	30.619380
458.168054	21139.228245	30.624397
458.250544	21162.453863	30.629415
458.718191	21185.613230	30.634432
459.251788	21236.664003	30.639450
460.063872	21260.881860	30.644468
460.554403	21297.401047	30.649485
461.170788	21324.044096	30.654503
461.572595	21345.665909	30.659520
462.128659	21388.215403	30.664538
462.546939	21415.022102	30.669556
463.128882	21448.658800	30.674573
463.105375	21471.825465	30.679591
463.855763	21504.014397	30.684608
464.032457	21551.753844	30.689626
464.577366	21579.570955	30.694644
465.109420	21611.465495	30.699661
465.773447	21646.530356	30.704679
466.740481	21671.501767	30.709696
466.575596	21706.240848	30.714714
467.199973	21729.793477	30.719732
467.975955	21766.307007	30.724749
468.345336	21790.904044	30.729767
468.606772	21824.471229	30.734784
468.799162	21859.464567	30.739802
469.797175	21888.058257	30.744820
469.935010	21930.844633	30.749837
470.585846	21953.982706	30.754855
470.793688	21979.710872	30.759872
471.444418	22019.776441	30.764890
472.471235	22042.198955	30.769908
472.816838	22070.028832	30.774925
473.089596	22099.171718	30.779943
474.011055	22125.187050	30.784960
474.042953	22157.501542	30.789978
474.362331	22170.095169	30.794996
474.525025	22203.229750	30.800013
475.007921	22240.958732	30.805031
476.003526	22271.006640	30.810048
476.091744	22317.068316	30.815066
476.473714	22344.583304	30.820084
476.926212	22391.492012	30.825101
476.960714	22429.954622	30.830119
477.719650	22456.084155	30.835136
477.967927	22500.143585	30.840154
478.672929	22547.392476	30.845172
479.423819	22582.988891	30.850189
479.706552	22611.909824	30.855207
480.291888	22649.794245	30.860224
480.479965	22687.658440	30.865242
480.946836	22723.191903	30.870260
481.582899	22755.388041	30.875277
482.029270	22791.013281	30.880295
482.391266	22819.726295	30.885312
482.940505	22859.771455	30.890330
483.316897	22893.543718	30.895348
484.367797	22920.203428	30.900365
484.674680	22954.182500	30.905383
485.424431	22981.179842	30.910400
485.923617	23015.306011	30.915418
485.858854	23042.575572	30.920436
486.554050	23071.793141	30.925453
486.676232	23099.855135	30.930471
487.750753	23121.728028	30.935488
488.222821	23162.544083	30.940506
488.344824	23191.181256	30.945524
488.771615	23221.439223	30.950541
488.989330	23263.242925	30.955559
489.736615	23303.346615	30.960576
489.917753	23344.183060	30.965594
490.494841	23377.634230	30.970612
491.128430	23423.841058	30.975629
491.252312	23468.648691	30.980647
492.549794	23509.324323	30.985664
492.546909	23538.802914	30.990682
493.142122	23581.439502	30.995700
493.852214	23612.412249	31.000717
494.218668	23651.109904	31.005735
495.300941	23678.347109	31.010752
495.491042	23717.122900	31.015770
495.833855	23751.906588	31.020788
496.441225	23778.175207	31.025805
497.138555	23823.772725	31.030823
497.625185	23853.295638	31.035840
497.991403	23892.480374	31.040858
498.393056	23925.713332	31.045876
499.030014	23959.453163	31.050893
499.612058	23999.546069	31.055911
500.134771	24038.972137	31.060928
500.430401	24078.800148	31.065946
501.153419	24110.542604	31.070964
501.516542	24142.221072	31.075981
502.605471	24157.944251	31.080999
503.616570	24181.723964	31.086016
504.084616	24204.956319	31.091034
504.310487	24234.128598	31.096052
505.486208	24250.912615	31.101069
505.354050	24277.556112	31.106087
505.828410	24309.381830	31.111104
506.283998	24334.189780	31.116122
506.643693	24359.031646	31.121140
506.997212	24391.084844	31.126157
507.080810	24438.498167	31.131175
507.822587	24460.626560	31.136192
508.384386	24499.914749	31.141210
508.217488	24543.758969	31.146228
509.312560	24560.985521	31.151245
509.642376	24612.601225	31.156263
510.101428	24652.354385	31.161280
510.662710	24687.762913	31.166298
510.730011	24728.992759	31.171316
511.760298	24763.121399	31.176333
511.739028	24805.161439	31.181351
512.287850	24849.432060	31.186368
512.172046	24894.779444	31.191386
512.756480	24936.390534	31.196404
513.914355	24987.258984	31.201421
514.452387	25027.196498	31.206439
514.569429	25080.148350	31.211456
515.382298	25114.848597	31.216474
515.785674	25168.495494	31.221492
516.549955	25203.323531	31.226509
516.972614	25230.621311	31.231527
517.525073	25271.290137	31.236544
517.934159	25305.383698	31.241562
518.579332	25335.256978	31.246580
519.611987	25371.162099	31.251597
519.377134	25409.912533	31.256615
519.984597	25437.864347	31.261632
520.791541	25474.822255	31.266650
521.141335	25510.309398	31.271668
522.037261	25541.584835	31.276685
522.530272	25579.476562	31.281703
523.188443	25609.525179	31.286720
523.981031	25637.081910	31.291738
524.445225	25664.266380	31.296756
524.960645	25695.708728	31.301773
525.323068	25727.168623	31.306791
525.900839	25764.617763	31.311808
526.632225	25780.467407	31.316826
526.880097	25821.405957	31.321844
528.010376	25840.859016	31.326861
528.395103	25870.792599	31.331879
528.705238	25900.346011	31.336896
530.036018	25913.302783	31.341914
530.293132	25940.481946	31.346932
530.944677	25968.623552	31.351949
531.281065	25995.392300	31.356967
531.875100	26017.494859	31.361984
532.258499	26047.100281	31.367002
532.365631	26078.543590	31.372020
533.101630	26098.930420	31.377037
533.466854	26126.105643	31.382055
533.698561	26172.179151	31.387072
534.195717	26204.844876	31.392090
534.463700	26249.509898	31.397108
535.383213	26286.236900	31.402125
535.358395	26329.374023	31.407143
536.055190	26371.406671	31.412160
536.677041	26405.620653	31.417178
537.043166	26451.793954	31.422196
537.676233	26491.011748	31.427213
538.000645	26538.114455	31.432231
538.853528	26579.137318	31.437248
539.502214	26615.414121	31.442266
539.744408	26663.888725	31.447284
540.370766	26701.970368	31.452301
541.135482	26742.988329	31.457319
541.493025	26790.914396	31.462336
542.272041	26826.912167	31.467354
542.785636	26868.961731	31.472372
543.264222	26901.530352	31.477389
544.260323	26945.672758	31.482407
544.379235	26982.715266	31.487424
545.048828	27022.648901	31.492442
545.362604	27062.764410	31.497460
545.698263	27100.474929	31.502477
546.527542	27150.843837	31.507495
546.471757	27185.840892	31.512512
547.446612	27233.937356	31.517530
547.999292	27280.348954	31.522548
548.341529	27316.700003	31.527565
548.976390	27369.122195	31.532583
549.593120	27407.023377	31.537600
550.633305	27435.928164	31.542618
550.870069	27471.505876	31.547636
551.780713	27509.203488	31.552653
552.844066	27538.085854	31.557671
553.376768	27572.195604	31.562688
553.897857	27597.819027	31.567706
554.270133	27630.689786	31.572724
554.858534	27656.492414	31.577741
555.709828	27679.201421	31.582759
556.049825	27709.132051	31.587776
556.531414	27734.477379	31.592794
556.935331	27761.509730	31.597812
557.376396	27794.401647	31.602829
557.922262	27822.998398	31.607847
558.089836	27859.605144	31.612864
558.679830	27892.316026	31.617882
559.198699	27941.698675	31.622900
559.583097	27972.848945	31.627917
560.096571	28020.165841	31.632935
560.460358	28058.682779	31.637952
561.157427	28092.856304	31.642970
562.404256	28125.869820	31.647988
562.767085	28157.523048	31.653005
563.842397	28194.115495	31.658023
564.213384	28225.103905	31.663040
564.696680	28255.651404	31.668058
565.216106	28294.093995	31.673076
565.589180	28333.558089	31.678093
566.517249	28367.626589	31.683111
567.003564	28397.503851	31.688128
567.887474	28433.532393	31.693146
568.139696	28471.460704	31.698164
568.721946	28508.794137	31.703181
569.262461	28554.376220	31.708199
569.404210	28584.357962	31.713216
569.751244	28610.553332	31.718234
570.312547	28662.358247	31.723252
571.341156	28707.144134	31.728269
571.741380	28752.343976	31.733287
571.813568	28802.076357	31.738304
572.610856	28845.293102	31.743322
573.250959	28895.973898	31.748340
573.927804	28938.116104	31.753357
574.636932	28979.994220	31.758375
575.184519	29024.969461	31.763392
575.785709	29063.046809	31.768410
576.074285	29106.090468	31.773428
576.766965	29140.588794	31.778445
577.943454	29181.174653	31.783463
578.767947	29223.616824	31.788480
579.354581	29255.894282	31.793498
580.116899	29299.028939	31.798516
580.453611	29329.190009	31.803533
581.224387	29363.562779	31.808551
581.457644	29395.092718	31.813568
582.091354	29430.757435	31.818586
582.723388	29467.206267	31.823604
583.264325	29505.382312	31.828621
583.786127	29550.324796	31.833639
584.359594	29588.818299	31.838656
584.799971	29616.574341	31.843674
585.333348	29666.881763	31.848692
585.791647	29704.236676	31.853709
586.260339	29742.026187	31.858727
586.624960	29791.412037	31.863744
587.440793	29836.890908	31.868762
587.540239	29895.780849	31.873780
588.213875	29938.873769	31.878797
588.826534	29986.679140	31.883815
589.262533	30028.355399	31.888832
590.124542	30075.388915	31.893850
590.667598	30117.301531	31.898868
591.383111	30158.327714	31.903885
592.078353	30202.176357	31.908903
592.363050	30254.104211	31.913920
593.038790	30287.020498	31.918938
593.731664	30331.546149	31.923956
594.177271	30384.252069	31.928973
594.583519	30417.937455	31.933991
595.054720	30465.759639	31.939008
595.737331	30497.815510	31.944026
596.246032	30549.525921	31.949044
597.049729	30595.141106	31.954061
597.376081	30641.582931	31.959079
597.899376	30705.485176	31.964096
598.684393	30745.389165	31.969114
599.173514	30792.975431	31.974132
599.603019	30850.476600	31.979149
600.585819	30891.601704	31.984167
600.937156	30949.608382	31.989184
601.408699	30999.138515	31.994202
602.289190	31046.835118	31.999220
602.616571	31099.814125	32.004237
603.414562	31146.392269	32.009255
603.668044	31207.411254	32.014272
604.561170	31256.440196	32.019290
605.142983	31314.601662	32.024308
605.518109	31369.849655	32.029325
606.567036	31427.338180	32.034343
607.188296	31481.644180	32.039360
607.663485	31530.346899	32.044378
608.794405	31587.861035	32.049396
609.516964	31632.087757	32.054413
610.264168	31679.332450	32.059431
610.856773	31727.309336	32.064448
611.498320	31768.938145	32.069466
611.943604	31817.665158	32.074484
612.219960	31867.689232	32.079501
613.288611	31899.952693	32.084519
613.628995	31959.550636	32.089536
614.386090	32003.127963	32.094554
615.552180	32045.693460	32.099572
616.049973	32085.246481	32.104589
616.902047	32122.816304	32.109607
616.976780	32186.369391	32.114624
617.809661	32221.388401	32.119642
618.411083	32266.570951	32.124660
618.612528	32316.588801	32.129677
619.542718	32357.876734	32.134695
619.787315	32413.988622	32.139712
620.616748	32460.002184	32.144730
621.169744	32503.011761	32.149748
621.746297	32555.721786	32.154765
622.588391	32609.661301	32.159783
623.055222	32660.795564	32.164800
624.052854	32701.232871	32.169818
624.470700	32751.515205	32.174836
625.244511	32802.266967	32.179853
625.842281	32844.941540	32.184871
626.250992	32896.565895	32.189888
626.729291	32940.005250	32.194906
627.604940	32993.125002	32.199924
628.168343	33035.729451	32.204941
629.226526	33079.249518	32.209959
629.857877	33125.535623	32.214976
630.285707	33177.960594	32.219994
630.794770	33212.633393	32.225012
631.405291	33253.637798	32.230029
632.190083	33295.778414	32.235047
633.046220	33339.520139	32.240064
634.047790	33377.334482	32.245082
634.690885	33410.241848	32.250100
635.308188	33444.354481	32.255117
635.828254	33473.987280	32.260135
636.252975	33511.860055	32.265152
636.790623	33543.209834	32.270170
637.257063	33585.337371	32.275188
637.916716	33619.241389	32.280205
638.589728	33643.369302	32.285223
638.794634	33706.021642	32.290240
639.177250	33740.215548	32.295258
640.495634	33781.667148	32.300276
640.692666	33822.338736	32.305293
641.560550	33861.104133	32.310311
642.025840	33914.347008	32.315328
642.585948	33959.128706	32.320346
642.926693	34006.113191	32.325364
643.592148	34059.755189	32.330381
644.665010	34106.467871	32.335399
645.350112	34156.206192	32.340416
646.082507	34190.694109	32.345434
647.026405	34233.785486	32.350452
647.520923	34273.197747	32.355469
648.206323	34317.644588	32.360487
649.211734	34365.519020	32.365504
649.851316	34392.479109	32.370522
650.631745	34431.923028	32.375540
651.134099	34481.412381	32.380557
652.140903	34517.742201	32.385575
652.291017	34564.795545	32.390592
652.860302	34603.507639	32.395610
653.644169	34636.957716	32.400628
654.448405	34691.426934	32.405645
655.033352	34723.700520	32.410663
655.607137	34783.232235	32.415680
655.844661	34828.078647	32.420698
656.574367	34876.389158	32.425716
657.033651	34921.567955	32.430733
657.819494	34974.687741	32.435751
657.822541	35036.066691	32.440768
658.688263	35086.607353	32.445786
659.163352	35140.711678	32.450804
659.735405	35196.014993	32.455821
660.875602	35257.268145	32.460839
661.190023	35311.296755	32.465856
661.937335	35373.755809	32.470874
662.243018	35429.398367	32.475892
663.151104	35491.314279	32.480909
663.730297	35549.089592	32.485927
664.416683	35610.983461	32.490944
665.124578	35671.249209	32.495962
665.988535	35734.392998	32.500980
666.822492	35788.070067	32.505997
667.624148	35835.593865	32.511015
668.544129	35901.650578	32.516032
668.982004	35948.750724	32.521050
669.800149	35999.553889	32.526068
670.204911	36058.849944	32.531085
671.085574	36112.217065	32.536103
671.556023	36166.874826	32.541120
672.119585	36221.227377	32.546138
673.087545	36275.643574	32.551156
673.745475	36334.907312	32.556173
674.081095	36384.755868	32.561191
674.887249	36443.933606	32.566208
675.163039	36504.509259	32.571226
676.267121	36553.909788	32.576244
676.767282	36609.000350	32.581261
677.807466	36655.831255	32.586279
678.620476	36710.980872	32.591296
678.914448	36756.435913	32.596314
679.915173	36806.940693	32.601332
680.941191	36846.540579	32.606349
681.530525	36881.573657	32.611367
682.028190	36931.821918	32.616384
682.327774	36975.284758	32.621402
683.495484	37026.181393	32.626420
683.848239	37070.749031	32.631437
684.349343	37118.847312	32.636455
685.370488	37175.963866	32.641472
685.636563	37228.126875	32.646490
686.304453	37286.860558	32.651508
686.703346	37336.524438	32.656525
687.357361	37391.061914	32.661543
688.064682	37447.507193	32.666560
688.313755	37504.302182	32.671578
689.477530	37558.855582	32.676596
690.216003	37619.710157	32.681613
690.599070	37679.595844	32.686631
691.378665	37744.213103	32.691648
692.506054	37796.515322	32.696666
693.847059	37850.523358	32.701684
694.227971	37909.372981	32.706701
695.197123	37954.346057	32.711719
695.889430	38002.062445	32.716736
696.782064	38052.536411	32.721754
697.944703	38104.106695	32.726772
698.043905	38154.413533	32.731789
698.510499	38200.837561	32.736807
699.373094	38255.654623	32.741824
699.948729	38314.127248	32.746842
700.629128	38368.966637	32.751860
701.026624	38420.416495	32.756877
702.119002	38467.793402	32.761895
702.691327	38523.680757	32.766912
703.407644	38586.274196	32.771930
704.073247	38637.701808	32.776948
704.443437	38699.381938	32.781965
704.987478	38756.090054	32.786983
705.962825	38825.675811	32.792000
706.887455	38882.818265	32.797018
707.787977	38932.420396	32.802036
708.051175	39006.278619	32.807053
708.827525	39047.078695	32.812071
709.597958	39107.654264	32.817088
710.532927	39169.247818	32.822106
711.305255	39226.478130	32.827124
711.870012	39290.482125	32.832141
712.610116	39340.533865	32.837159
713.423893	39409.900029	32.842176
713.888084	39466.356838	32.847194
714.404706	39512.541921	32.852212
715.353646	39581.634638	32.857229
716.195990	39644.078725	32.862247
716.753070	39704.594321	32.867264
717.200951	39776.959265	32.872282
717.900628	39833.481558	32.877300
718.525708	39895.922248	32.882317
719.311271	39955.277299	32.887335
720.558628	40017.008038	32.892352
720.786946	40081.730771	32.897370
722.228037	40133.091816	32.902388
722.582116	40197.042750	32.907405
723.324908	40262.609255	32.912423
724.408348	40310.750497	32.917440
725.087620	40364.595914	32.922458
726.392367	40406.859396	32.927476
726.859226	40454.401280	32.932493
727.797834	40494.951158	32.937511
728.736933	40532.813247	32.942528
729.586042	40573.484716	32.947546
730.366890	40598.817979	32.952564
730.788604	40632.637385	32.957581
731.383533	40677.604830	32.962599
731.960919	40716.048458	32.967616
732.284021	40769.703677	32.972634
733.388422	40815.066418	32.977652
733.521932	40868.662853	32.982669
733.939175	40911.868662	32.987687
734.673154	40971.987116	32.992704
734.854426	41038.389643	32.997722
736.378751	41095.748151	33.002740
736.693711	41171.066610	33.007757
737.440343	41223.278296	33.012775
738.076930	41292.013991	33.017792
739.088810	41359.243182	33.022810
739.657662	41427.673626	33.027828
739.984817	41500.708189	33.032845
741.085610	41558.956030	33.037863
741.838118	41626.694433	33.042880
742.342192	41690.411362	33.047898
743.458073	41754.336816	33.052916
743.959584	41828.123251	33.057933
744.659328	41895.010554	33.062951
745.545416	41956.689189	33.067968
746.365323	42039.401410	33.072986
746.968059	42097.816761	33.078004
748.136723	42175.504021	33.083021
749.142481	42238.998980	33.088039
749.635071	42293.118551	33.093056
750.423140	42359.955575	33.098074
751.303801	42410.232832	33.103092
751.976106	42478.637802	33.108109
752.729176	42551.135202	33.113127
753.914223	42609.644687	33.118144
754.631974	42678.138074	33.123162
755.379908	42727.247651	33.128180
756.606125	42783.044157	33.133197
757.642909	42835.208191	33.138215
758.440277	42879.010168	33.143232
759.403088	42934.544468	33.148250
760.398160	42976.412068	33.153268
760.893018	43018.332314	33.158285
761.346897	43072.276405	33.163303
762.647122	43115.077132	33.168320
762.985404	43173.669333	33.173338
763.684178	43222.692793	33.178356
764.254106	43285.265595	33.183373
764.809914	43328.024492	33.188391
765.703374	43396.176509	33.193408
766.202996	43461.208541	33.198426
766.862782	43507.133101	33.203444
767.498601	43576.540193	33.208461
768.204142	43642.527417	33.213479
768.989419	43703.094446	33.218496
769.760565	43780.343238	33.223514
770.205132	43833.215360	33.228532
771.061272	43897.965472	33.233549
771.615572	43975.963446	33.238567
772.828183	44032.366125	33.243584
773.049822	44106.728743	33.248602
773.961186	44163.184975	33.253620
775.040894	44236.111451	33.258637
775.804535	44292.806068	33.263655
776.676466	44354.348132	33.268672
777.418662	44411.463860	33.273690
779.070705	44459.747087	33.278708
780.020622	44517.254550	33.283725
780.115586	44567.349084	33.288743
781.581056	44605.193191	33.293760
782.154043	44659.615984	33.298778
782.735928	44709.976614	33.303796
783.382514	44760.536024	33.308813
783.789691	44811.012634	33.313831
784.518219	44863.767101	33.318848
784.848395	44929.215663	33.323866
785.428807	44994.555883	33.328884
786.530316	45049.763949	33.333901
787.103062	45118.002805	33.338919
787.731078	45182.558126	33.343936
788.740102	45256.258016	33.348954
789.328120	45312.419593	33.353972
789.965473	45392.648857	33.358989
790.774949	45472.807336	33.364007
791.617009	45538.443676	33.369024
792.701484	45610.197341	33.374042
793.717962	45674.193884	33.379060
795.122217	45750.566575	33.384077
795.564846	45824.179386	33.389095
796.443426	45874.325661	33.394112
797.094074	45939.600778	33.399130
798.193028	46006.495281	33.404148
799.322257	46074.650430	33.409165
799.958040	46128.048572	33.414183
800.963473	46173.874222	33.419200
801.640691	46249.988568	33.424218
802.705734	46296.349212	33.429236
803.321939	46355.450540	33.434253
803.920445	46417.338170	33.439271
805.086449	46475.531863	33.444288
805.904597	46538.049856	33.449306
806.689950	46594.493898	33.454324
807.336470	46649.643894	33.459341
807.850866	46731.282470	33.464359
808.813289	46786.389952	33.469376
809.607535	46856.832696	33.474394
810.389750	46916.150044	33.479412
810.636176	46981.813738	33.484429
811.398197	47068.652957	33.489447
812.159805	47130.574092	33.494464
813.503825	47208.808338	33.499482
815.168744	47259.012430	33.504500
815.879925	47327.394605	33.509517
816.552475	47389.779471	33.514535
817.302602	47447.236992	33.519552
817.648270	47509.723683	33.524570
818.594478	47578.905090	33.529588
819.481608	47648.222431	33.534605
820.598511	47707.382212	33.539623
821.602190	47767.236684	33.544640
822.128091	47828.095651	33.549658
822.889567	47888.222218	33.554676
823.917158	47944.916612	33.559693
824.430028	48024.124462	33.564711
825.658930	48070.089996	33.569728
826.283914	48147.844744	33.574746
827.307255	48211.790494	33.579764
827.825463	48264.028957	33.584781
828.977976	48321.603198	33.589799
829.291157	48385.584068	33.594816
830.290689	48456.404728	33.599834
831.121681	48517.496416	33.604852
832.248597	48576.941599	33.609869
832.695381	48632.127520	33.614887
833.248824	48689.473296	33.619904
834.249523	48748.558985	33.624922
834.927572	48809.953633	33.629940
836.098770	48867.589615	33.634957
836.573684	48933.925640	33.639975
837.466616	48990.523402	33.644992
838.271941	49052.790944	33.650010
839.026991	49120.323922	33.655028
839.424438	49185.363122	33.660045
840.176234	49255.978092	33.665063
841.337339	49313.262478	33.670080
842.138661	49382.282129	33.675098
842.884581	49453.512316	33.680116
843.480803	49522.374514	33.685133
844.282300	49609.520982	33.690151
845.018485	49674.053313	33.695168
845.622982	49762.439447	33.700186
846.370589	49830.323655	33.705204
847.897541	49911.929919	33.710221
848.250732	49994.263298	33.715239
849.530185	50073.801812	33.720256
850.166774	50148.258919	33.725274
850.975041	50239.525557	33.730292
851.907071	50313.367784	33.735309
852.615353	50394.274367	33.740327
853.699777	50462.981141	33.745344
855.063861	50546.335962	33.750362
855.911029	50619.515388	33.755380
856.879359	50686.058066	33.760397
857.676285	50764.864219	33.765415
858.336389	50830.556846	33.770432
859.697441	50913.603440	33.775450
860.470698	50990.832265	33.780468
861.228120	51066.254241	33.785485
861.830522	51137.904274	33.790503
863.177716	51213.943572	33.795520
863.833099	51292.552107	33.800538
864.638420	51369.226736	33.805556
865.809707	51440.365225	33.810573
866.218467	51518.532045	33.815591
866.950227	51591.232660	33.820608
868.325528	51669.091349	33.825626
869.113079	51744.852523	33.830644
870.499955	51809.896976	33.835661
871.042750	51890.916818	33.840679
872.518003	51939.800348	33.845696
873.872537	52002.173878	33.850714
874.703889	52062.509320	33.855732
875.708400	52123.861997	33.860749
876.422146	52183.292250	33.865767
877.348975	52236.880841	33.870784
878.396935	52295.942983	33.875802
878.714208	52361.364289	33.880820
879.842869	52423.046444	33.885837
880.291302	52494.920792	33.890855
880.974299	52557.925538	33.895872
881.845377	52629.892702	33.900890
882.760429	52693.348917	33.905908
883.448522	52767.217965	33.910925
884.373438	52848.744820	33.915943
885.242350	52915.201807	33.920960
886.026107	52997.839518	33.925978
886.693477	53071.959537	33.930996
887.393358	53133.444555	33.936013
888.274102	53202.026637	33.941031
889.152419	53283.201581	33.946048
890.164299	53366.469502	33.951066
890.927170	53447.125122	33.956084
892.047673	53499.939786	33.961101
892.768064	53568.965543	33.966119
894.011656	53638.827602	33.971136
894.829420	53703.763446	33.976154
895.298059	53764.071161	33.981172
896.106977	53832.109414	33.986189
897.049792	53911.460379	33.991207
897.642912	53989.030935	33.996224
898.693597	54052.317854	34.001242
899.228314	54137.643451	34.006260
900.573145	54221.096715	34.011277
901.459177	54297.692473	34.016295
901.998289	54378.537997	34.021312
903.066838	54460.250600	34.026330
903.840346	54544.217927	34.031348
904.952054	54625.513056	34.036365
905.751812	54708.521333	34.041383
906.587294	54802.535389	34.046400
907.983869	54873.212626	34.051418
908.721257	54960.756168	34.056436
909.405533	55042.884987	34.061453
910.551921	55128.745453	34.066471
911.238715	55209.286060	34.071488
912.319169	55295.208019	34.076506
912.882139	55376.496227	34.081524
914.301005	55457.651483	34.086541
915.067106	55529.903335	34.091559
915.914362	55625.792031	34.096576
917.406552	55696.899837	34.101594
917.666182	55794.013473	34.106612
918.672369	55873.949716	34.111629
919.952549	55966.747388	34.116647
920.918516	56058.012203	34.121664
922.018436	56138.181558	34.126682
922.584701	56222.389607	34.131700
923.557436	56294.991336	34.136717
924.592641	56387.385781	34.141735
925.224889	56483.077244	34.146752
926.653387	56549.881388	34.151770
927.441864	56653.067657	34.156788
928.397381	56725.799952	34.161805
929.684431	56817.017693	34.166823
930.508948	56892.384651	34.171840
931.454269	56967.074851	34.176858
932.633510	57053.639649	34.181876
933.814863	57130.413762	34.186893
934.006677	57203.880286	34.191911
934.984285	57290.477327	34.196928
936.044740	57366.429279	34.201946
937.110899	57446.443733	34.206964
938.289423	57530.649691	34.211981
939.239931	57611.366220	34.216999
940.501224	57696.268717	34.222016
941.565826	57764.417681	34.227034
942.305807	57841.895676	34.232052
943.224754	57906.320950	34.237069
944.371969	57979.349992	34.242087
945.467175	58050.330411	34.247104
946.777066	58117.144738	34.252122
947.646385	58189.818946	34.257140
948.651970	58254.535463	34.262157
949.448487	58310.911272	34.267175
950.385441	58382.771736	34.272192
951.272575	58448.197088	34.277210
951.638486	58524.843098	34.282228
952.753304	58597.056265	34.287245
953.778710	58665.137931	34.292263
954.723395	58737.042551	34.297280
955.422931	58801.884129	34.302298
956.412950	58881.067086	34.307316
957.385912	58929.517949	34.312333
958.110485	58994.558683	34.317351
959.200648	59063.758007	34.322368
960.373758	59123.849367	34.327386
960.992267	59195.730172	34.332404
962.110796	59250.754204	34.337421
962.645994	59323.901572	34.342439
963.196546	59407.578899	34.347456
964.335455	59483.291124	34.352474
965.263537	59565.315214	34.357492
966.395545	59640.680884	34.362509
967.458545	59714.905564	34.367527
968.666305	59804.596242	34.372544
969.607450	59865.263556	34.377562
970.625404	59954.876732	34.382580
971.473169	60034.370428	34.387597
972.772430	60107.774664	34.392615
973.269466	60193.735348	34.397632
974.437631	60273.774935	34.402650
975.389502	60350.848198	34.407668
976.091854	60430.403799	34.412685
976.894569	60524.875783	34.417703
977.689361	60601.265362	34.422720
978.817754	60685.730633	34.427738
979.413480	60779.248381	34.432756
980.293167	60880.033188	34.437773
981.707618	60960.732966	34.442791
982.381059	61067.658915	34.447808
983.454802	61162.679847	34.452826
984.263666	61252.222719	34.457844
985.695315	61341.542377	34.462861
987.256632	61428.867238	34.467879
988.323215	61521.510621	34.472896
989.255945	61597.058937	34.477914
990.170694	61670.344148	34.482932
991.120701	61757.322234	34.487949
992.478069	61847.959279	34.492967
993.119946	61933.466742	34.497984
994.557501	62018.413871	34.503002
995.476768	62114.076543	34.508020
996.070909	62198.845403	34.513037
996.953829	62284.734351	34.518055
997.904735	62379.437274	34.523072
998.964980	62453.949210	34.528090
999.889890	62554.695854	34.533108
1000.963888	62642.107204	34.538125
1002.120863	62734.133368	34.543143
1002.686972	62828.613045	34.548160
1003.958016	62915.925055	34.553178
1004.955262	63006.090660	34.558196
1005.482480	63110.060302	34.563213
1006.833515	63194.670440	34.568231
1007.769147	63299.830718	34.573248
1008.894443	63384.413337	34.578266
1010.377735	63481.671058	34.583284
1010.835367	63581.348793	34.588301
1012.321274	63675.125100	34.593319
1013.368399	63763.582783	34.598336
1014.304930	63845.100723	34.603354
1015.612393	63933.201957	34.608372
1016.881849	64010.116937	34.613389
1018.431866	64075.878269	34.618407
1019.320720	64157.417313	34.623424
1020.389998	64234.731321	34.628442
1021.228101	64316.392735	34.633460
1022.154510	64397.610184	34.638477
1023.086735	64461.620137	34.643495
1023.876268	64537.756801	34.648512
1024.755679	64609.448189	34.653530
1026.018485	64676.585265	34.658548
1026.974833	64747.815589	34.663565
1028.232632	64799.215475	34.668583
1029.098203	64875.423630	34.673600
1030.247262	64947.111995	34.678618
1031.120886	65033.872863	34.683636
1031.874297	65114.005333	34.688653
1032.993906	65187.908442	34.693671
1034.154742	65265.736843	34.698688
1034.937989	65335.634635	34.703706
1035.836607	65422.728493	34.708724
1036.243257	65501.181492	34.713741
1037.265807	65594.372364	34.718759
1038.129957	65693.273483	34.723776
1039.421935	65779.161429	34.728794
1040.278199	65885.693426	34.733812
1041.053824	65982.488553	34.738829
1042.403591	66071.008558	34.743847
1042.831454	66177.969343	34.748864
1044.224579	66273.472879	34.753882
1045.419604	66375.883275	34.758900
1046.070532	66480.620026	34.763917
1047.364864	66573.082096	34.768935
1048.587870	66679.731289	34.773952
1049.920587	66775.815935	34.778970
1050.765353	66890.831533	34.783988
1051.866388	66988.789127	34.789005
1052.797679	67082.468196	34.794023
1053.679754	67192.078700	34.799040
1055.089873	67292.863801	34.804058
1056.229953	67405.176561	34.809076
1057.395758	67508.596435	34.814093
1058.436003	67606.166982	34.819111
1059.436104	67718.287637	34.824128
1060.879488	67812.795084	34.829146
1061.537968	67911.135352	34.834164
1061.908045	68031.054627	34.839181
1063.529126	68131.196034	34.844199
1064.720055	68239.040751	34.849216
1065.682360	68345.167635	34.854234
1067.197797	68443.503186	34.859252
1068.354018	68546.890755	34.864269
1069.192028	68645.509814	34.869287
1070.370827	68760.494485	34.874304
1071.756536	68861.789773	34.879322
1072.537066	68958.931007	34.884340
1073.968525	69059.871703	34.889357
1074.877304	69147.654215	34.894375
1075.940034	69255.466161	34.899392
1076.766711	69362.207215	34.904410
1078.138518	69462.177322	34.909428
1079.425094	69558.995099	34.914445
1081.072198	69652.952048	34.919463
1081.998442	69747.566098	34.924480
1083.068267	69832.672755	34.929498
1083.963190	69930.635664	34.934516
1084.436378	70028.816558	34.939533
1085.975693	70123.539179	34.944551
1087.046862	70215.460229	34.949568
1088.298402	70314.135263	34.954586
1089.755113	70403.065179	34.959604
1090.602370	70499.289972	34.964621
1091.644843	70582.035101	34.969639
1092.585606	70681.241151	34.974656
1093.736471	70766.002642	34.979674
1094.869694	70864.140939	34.984692
1095.989861	70936.395170	34.989709
1097.324938	71016.835503	34.994727
1098.543100	71092.139757	34.999744
1099.509619	71172.144014	35.004762
1100.557755	71243.663090	35.009780
1101.627412	71332.757745	35.014797
1102.780674	71413.265594	35.019815
1103.809991	71496.237305	35.024832
1104.509803	71585.732341	35.029850
1105.739450	71664.379995	35.034868
1106.625233	71757.633493	35.039885
1107.645965	71850.942307	35.044903
1108.819841	71945.316813	35.049920
1109.479277	72039.087816	35.054938
1110.838531	72137.993609	35.059956
1111.617929	72236.014809	35.064973
1112.589187	72322.151810	35.069991
1113.461595	72441.360973	35.075008
1114.458209	72553.319406	35.080026
1115.759332	72656.795734	35.085044
1116.843353	72771.502552	35.090061
1117.998639	72876.522300	35.095079
1119.446648	72981.167597	35.100096
1119.959958	73098.168478	35.105114
1121.149159	73207.186604	35.110132
1122.504296	73316.217347	35.115149
1124.359210	73417.026636	35.120167
1125.342215	73526.660798	35.125184
1126.802812	73638.488270	35.130202
1127.834156	73743.467417	35.135220
1128.960991	73845.772254	35.140237
1130.111305	73950.569041	35.145255
1131.540070	74057.780123	35.150272
1132.528330	74158.701794	35.155290
1134.030273	74250.284901	35.160308
1135.257277	74352.234104	35.165325
1136.714097	74436.516454	35.170343
1137.982948	74532.620678	35.175360
1139.254538	74623.265614	35.180378
1140.448468	74717.912867	35.185396
1141.003905	74809.252561	35.190413
1142.325413	74902.854626	35.195431
1143.429174	75002.900185	35.200448
1144.313311	75103.676966	35.205466
1145.405611	75199.583066	35.210484
1146.242102	75307.106681	35.215501
1147.438650	75409.077315	35.220519
1148.484206	75521.977946	35.225536
1149.515229	75623.544487	35.230554
1151.047166	75727.212146	35.235572
1151.853177	75836.414649	35.240589
1153.127912	75936.006391	35.245607
1154.028702	76048.716422	35.250624
1155.427902	76162.970732	35.255642
1157.051503	76262.699383	35.260660
1157.656545	76369.731241	35.265677
1158.864521	76480.381173	35.270695
1160.002564	76586.874904	35.275712
1161.022516	76699.961785	35.280730
1162.473037	76800.682078	35.285748
1163.304872	76909.504868	35.290765
1164.688348	77011.490455	35.295783
1166.081528	77119.023297	35.300800
1167.046249	77233.425753	35.305818
1168.278149	77338.058351	35.310836
1169.684973	77444.158910	35.315853
1170.802283	77533.342848	35.320871
1171.476737	77646.550780	35.325888
1172.977361	77746.126674	35.330906
1174.008578	77825.646746	35.335924
1174.729822	77931.729236	35.340941
1175.866250	78026.168993	35.345959
1177.465817	78116.698582	35.350976
1178.939146	78219.789487	35.355994
1180.005528	78305.588834	35.361012
1180.918076	78410.959325	35.366029
1182.132947	78515.003677	35.371047
1183.144024	78613.404775	35.376064
1184.110262	78718.071334	35.381082
1185.383595	78823.488596	35.386100
1186.325211	78936.140865	35.391117
1187.270215	79042.458852	35.396135
1188.668312	79155.116974	35.401152
1189.820409	79277.302578	35.406170
1191.507407	79378.983702	35.411188
1192.548437	79500.148756	35.416205
1193.839354	79611.368529	35.421223
1194.735783	79718.583488	35.426240
1196.048080	79827.925830	35.431258
1197.612063	79940.941397	35.436276
1198.665085	80073.027633	35.441293
1199.949681	80183.211835	35.446311
1201.229653	80288.899700	35.451328
1202.493556	80402.229903	35.456346
1203.991736	80516.220903	35.461364
1204.993454	80631.429869	35.466381
1206.253249	80740.125177	35.471399
1207.558552	80851.575722	35.476416
1208.446895	80964.345875	35.481434
1209.782747	81064.618192	35.486452
1211.115829	81185.073654	35.491469
1212.384477	81300.231161	35.496487
1213.925823	81413.205548	35.501504
1215.062757	81530.335607	35.506522
1216.215291	81638.214911	35.511540
1217.458792	81752.554666	35.516557
1218.692391	81864.780586	35.521575
1219.774348	81973.216960	35.526592
1220.802331	82095.852341	35.531610
1222.260427	82205.574063	35.536628
1223.301940	82330.425586	35.541645
1224.807050	82454.115883	35.546663
1225.626719	82560.314746	35.551680
1227.075266	82673.295970	35.556698
1228.233043	82786.322904	35.561716
1229.127067	82918.041848	35.566733
1230.325763	83033.559426	35.571751
1231.877897	83151.062379	35.576768
1232.765184	83279.945907	35.581786
1234.337266	83394.583265	35.586804
1235.396747	83519.335869	35.591821
1236.611142	83649.563907	35.596839
1237.724898	83769.887153	35.601856
1238.619030	83900.191527	35.606874
1240.393822	84009.541504	35.611892
1241.440451	84143.295015	35.616909
1242.886899	84270.613514	35.621927
1244.448053	84390.502285	35.626944
1245.149891	84506.711374	35.631962
1247.003287	84620.714343	35.636980
1248.290630	84741.128697	35.641997
1249.642906	84859.024583	35.647015
1251.239904	84969.711022	35.652032
1252.469240	85085.751652	35.657050
1253.690439	85195.711845	35.662068
1254.516231	85301.970645	35.667085
1255.872437	85399.619503	35.672103
1256.832686	85489.499446	35.677120
1257.914257	85609.049798	35.682138
1259.357470	85703.518300	35.687156
1261.084567	85819.598451	35.692173
1262.174827	85917.949375	35.697191
1263.030171	86024.117532	35.702208
1263.861004	86143.176914	35.707226
1265.438716	86255.252494	35.712244
1266.239217	86364.015450	35.717261
1267.487132	86486.977566	35.722279
1268.524485	86608.186252	35.727296
1269.738724	86739.163262	35.732314
1270.840833	86854.356430	35.737332
1272.313159	86984.584744	35.742349
1273.445197	87118.680888	35.747367
1275.068308	87241.651151	35.752384
1276.586751	87368.769342	35.757402
1277.655773	87496.870435	35.762420
1279.290457	87624.301120	35.767437
1280.623369	87751.259766	35.772455
1282.239964	87859.419721	35.777472
1283.831595	87980.966015	35.782490
1285.058758	88101.352987	35.787508
1286.657790	88215.029504	35.792525
1287.805243	88333.959824	35.797543
1289.391181	88438.160172	35.802560
1290.807544	88573.904169	35.807578
1292.054925	88675.889648	35.812596
1293.478233	88789.608407	35.817613
1294.400270	88911.985114	35.822631
1295.607446	89034.191216	35.827648
1297.088379	89155.341380	35.832666
1297.985035	89265.266032	35.837684
1299.573947	89380.900249	35.842701
1300.385114	89509.937336	35.847719
1301.761111	89625.466243	35.852736
1303.223886	89754.200197	35.857754
1304.234821	89881.750389	35.862772
1306.036986	90002.131634	35.867789
1307.084397	90132.490686	35.872807
1308.630317	90260.681608	35.877824
1309.856122	90388.846865	35.882842
1311.314433	90511.577577	35.887860
1312.731341	90633.656213	35.892877
1313.762499	90764.755616	35.897895
1315.248970	90878.130339	35.902912
1316.087294	91012.809458	35.907930
1317.710646	91135.174845	35.912948
1319.019711	91265.193928	35.917965
1320.509899	91397.035765	35.922983
1321.922216	91512.946522	35.928000
1322.993485	91643.967469	35.933018
1324.227714	91767.523975	35.938036
1325.682771	91893.974322	35.943053
1326.972465	92017.662632	35.948071
1328.312267	92153.041907	35.953088
1329.158284	92284.937186	35.958106
1330.425167	92416.856250	35.963124
1332.180412	92550.246143	35.968141
1333.548483	92688.120250	35.973159
1335.172445	92809.998019	35.978176
1336.073344	92939.352705	35.983194
1337.403385	93068.134161	35.988212
1339.047969	93199.186655	35.993229
1340.331387	93322.272867	35.998247
1341.866160	93446.625947	36.003264
1343.168085	93560.711195	36.008282
1344.415863	93673.791311	36.013300
1345.873511	93781.173521	36.018317
1347.250345	93889.240455	36.023335
1348.501913	93999.101758	36.028352
1349.554038	94112.340693	36.033370
1350.783794	94234.868547	36.038388
1352.523287	94337.303594	36.043405
1353.956783	94456.099495	36.048423
1355.414748	94565.144836	36.053440
1356.514204	94684.513291	36.058458
1357.180654	94796.623298	36.063476
1358.940118	94929.820092	36.068493
1360.213893	95056.970850	36.073511
1361.554797	95179.434451	36.078528
1363.273212	95303.563640	36.083546
1365.006899	95426.017780	36.088564
1366.157399	95548.436420	36.093581
1367.044337	95674.166875	36.098599
1368.692828	95795.773790	36.103616
1370.406035	95926.573684	36.108634
1371.337403	96049.142480	36.113652
1372.762347	96178.872830	36.118669
1373.889210	96322.834430	36.123687
1375.244415	96447.455691	36.128704
1376.872904	96584.241891	36.133722
1378.074578	96713.793719	36.138740
1379.476554	96844.367020	36.143757
1380.470257	96981.824180	36.148775
1381.981912	97131.116961	36.153792
1383.624694	97273.012450	36.158810
1384.852013	97411.195698	36.163828
1386.198544	97547.725743	36.168845
1387.181959	97692.920197	36.173863
1388.931678	97834.117035	36.178880
1390.675310	97984.074949	36.183898
1391.817607	98128.384664	36.188916
1393.603049	98261.071839	36.193933
1394.692299	98410.347667	36.198951
1396.560662	98552.885648	36.203968
1397.683699	98682.838086	36.208986
1399.275060	98824.533020	36.214004
1401.012424	98963.543699	36.219021
1402.216695	99113.185223	36.224039
1403.623139	99245.948167	36.229056
1405.548135	99378.288669	36.234074
1406.881471	99516.540625	36.239092
1408.383895	99643.826422	36.244109
1409.683274	99773.400880	36.249127
1411.261963	99915.673090	36.254144
1412.330253	100047.236927	36.259162
1413.896160	100191.439305	36.264180
1415.376800	100319.352359	36.269197
1416.282934	100464.000939	36.274215
1417.965874	100599.376038	36.279232
1419.628357	100743.832079	36.284250
1420.698849	100882.713975	36.289268
1421.887276	101018.231182	36.294285
1423.360823	101156.582437	36.299303
1424.670429	101308.968836	36.304320
1425.905898	101453.355041	36.309338
1427.694794	101592.698657	36.314356
1429.265354	101737.325556	36.319373
1430.673255	101885.236681	36.324391
1432.008051	102024.373900	36.329408
1433.529029	102163.178455	36.334426
1434.801021	102314.725960	36.339444
1436.218550	102438.295845	36.344461
1437.547657	102573.822964	36.349479
1438.457270	102700.972117	36.354496
1440.064136	102831.728022	36.359514
1441.358916	102963.192304	36.364532
1442.636430	103094.330154	36.369549
1444.292860	103236.693508	36.374567
1445.452961	103385.676917	36.379584
1446.906681	103517.980816	36.384602
1448.082151	103674.151962	36.389620
1449.901091	103806.362130	36.394637
1451.289876	103948.034825	36.399655
1452.698586	104093.800318	36.404672
1454.283854	104238.714835	36.409690
1455.554652	104382.601208	36.414708
1457.522477	104532.833374	36.419725
1458.672545	104680.949285	36.424743
1460.050085	104828.878296	36.429760
1461.624110	104982.622521	36.434778
1463.051622	105133.575444	36.439796
1464.578539	105274.357386	36.444813
1465.747079	105436.433758	36.449831
1467.390594	105586.087147	36.454848
1468.855557	105743.186531	36.459866
1470.361734	105906.594682	36.464884
1472.038119	106062.077689	36.469901
1473.162612	106220.614369	36.474919
1474.720372	106375.242375	36.479936
1476.280201	106545.568424	36.484954
1477.677570	106700.184834	36.489972
1479.542836	106859.610910	36.494989
1480.789198	107010.942760	36.500007
1482.528621	107179.215219	36.505024
1484.183390	107338.955259	36.510042
1485.433417	107504.553898	36.515060
1486.891147	107658.746804	36.520077
1488.175871	107825.191167	36.525095
1490.116632	107979.842907	36.530112
1491.603468	108142.656119	36.535130
1492.873609	108309.903963	36.540148
1494.762914	108463.335874	36.545165
1496.070157	108632.227977	36.550183
1497.888161	108783.605464	36.555200
1499.661159	108943.195057	36.560218
1500.919354	109102.573851	36.565236
1502.677067	109264.361077	36.570253
1504.338126	109420.495729	36.575271
1506.023806	109558.430060	36.580288
1507.958710	109700.181175	36.585306
1509.625554	109853.882112	36.590324
1511.161192	109994.352371	36.595341
1512.986367	110139.863279	36.600359
1514.378254	110276.704866	36.605376
1515.973787	110422.810665	36.610394
1516.936787	110565.439386	36.615412
1519.016721	110699.499769	36.620429
1520.292762	110847.140778	36.625447
1521.845009	110998.936986	36.630464
1523.360353	111134.532587	36.635482
1525.100458	111266.479475	36.640500
1526.935735	111400.669372	36.645517
1528.305144	111537.874437	36.650535
1529.964035	111680.272528	36.655552
1531.405913	111814.309631	36.660570
1532.836394	111943.593329	36.665588
1534.188287	112083.174724	36.670605
1535.367471	112240.360694	36.675623
1536.868807	112373.173179	36.680640
1538.346591	112493.662901	36.685658
1539.498271	112638.274342	36.690676
1540.592828	112779.534495	36.695693
1542.052198	112911.061930	36.700711
1543.593390	113055.601745	36.705728
1545.078375	113186.783783	36.710746
1546.332042	113331.711879	36.715764
1547.608483	113475.051717	36.720781
1548.934147	113630.686405	36.725799
1550.485168	113780.668354	36.730816
1552.150407	113929.288799	36.735834
1553.519969	114098.438235	36.740852
1555.223989	114257.872233	36.745869
1556.425065	114422.382190	36.750887
1558.071606	114586.100640	36.755904
1559.793886	114754.767014	36.760922
1560.603540	114919.758668	36.765940
1562.556887	115089.506715	36.770957
1563.859080	115266.015463	36.775975
1565.402282	115445.239769	36.780992
1567.078472	115614.018736	36.786010
1568.894362	115802.879552	36.791028
1570.352032	115969.271671	36.796045
1571.967732	116144.936792	36.801063
1573.190685	116330.975438	36.806080
1575.924689	116510.666429	36.811098
1577.238735	116687.357694	36.816116
1578.808792	116857.909172	36.821133
1580.281261	117035.363810	36.826151
1582.066210	117226.900247	36.831168
1583.747167	117389.890123	36.836186
1585.276692	117564.915806	36.841204
1586.828705	117746.268038	36.846221
1588.694752	117919.657520	36.851239
1590.306600	118101.623664	36.856256
1591.807737	118268.463210	36.861274
1593.697681	118442.853418	36.866292
1595.341430	118624.449280	36.871309
1597.393090	118795.657597	36.876327
1598.694870	118969.177775	36.881344
1600.544018	119138.250153	36.886362
1602.007358	119312.330229	36.891380
1603.417432	119488.245945	36.896397
1604.989269	119659.989473	36.901415
1606.712651	119840.678148	36.906432
1608.607038	120015.100242	36.911450
1610.121445	120184.140556	36.916468
1612.307234	120352.886850	36.921485
1613.765437	120522.774591	36.926503
1615.336991	120693.964660	36.931520
1617.263688	120867.725980	36.936538
1618.744031	121034.783802	36.941556
1620.621846	121197.772029	36.946573
1622.345399	121362.890666	36.951591
1623.846417	121536.949571	36.956608
1625.855675	121697.902509	36.961626
1627.046131	121861.736239	36.966644
1628.643412	122023.503069	36.971661
1630.527529	122186.151951	36.976679
1631.754288	122355.880764	36.981696
1633.496563	122525.999435	36.986714
1634.993166	122688.380892	36.991732
1636.405294	122854.657933	36.996749
1638.306943	123020.326693	37.001767
1639.559855	123197.336578	37.006784
1641.294634	123359.747156	37.011802
1642.907587	123530.930513	37.016820
1643.927916	123714.550116	37.021837
1645.995481	123881.731635	37.026855
1647.315358	124049.055599	37.031872
1648.791537	124208.110071	37.036890
1650.450803	124365.246468	37.041908
1651.768402	124535.896555	37.046925
1652.815853	124706.323006	37.051943
1654.500885	124890.884817	37.056960
1656.389006	125058.974529	37.061978
1657.604475	125233.956787	37.066996
1658.991432	125417.298775	37.072013
1660.908160	125599.823328	37.077031
1662.525304	125792.278071	37.082048
1664.292631	125970.628334	37.087066
1665.595838	126166.381453	37.092084
1667.041938	126361.745359	37.097101
1669.067541	126563.350661	37.102119
1670.394305	126771.980001	37.107136
1672.141406	126966.361126	37.112154
1673.539360	127174.917999	37.117172
1675.725484	127377.225467	37.122189
1677.339472	127582.718602	37.127207
1678.946849	127784.648724	37.132224
1680.700048	127990.274460	37.137242
1682.591028	128200.168039	37.142260
1684.555696	128388.178396	37.147277
1686.574130	128590.276826	37.152295
1688.263265	128789.661640	37.157312
1690.234940	128981.023039	37.162330
1692.369577	129182.789060	37.167348
1693.512974	129376.070108	37.172365
1695.957299	129572.486406	37.177383
1697.617508	129769.101785	37.182400
1699.373868	129963.152881	37.187418
1700.958058	130163.118791	37.192436
1702.681508	130353.205520	37.197453
1704.476668	130539.171060	37.202471
1706.574476	130736.446021	37.207488
1708.151862	130917.371925	37.212506
1709.608501	131113.885634	37.217524
1711.364164	131313.436915	37.222541
1713.352672	131502.662773	37.227559
1714.979118	131698.987782	37.232576
1716.667210	131900.112951	37.237594
1718.183645	132099.197571	37.242612
1719.890259	132296.109165	37.247629
1721.528081	132491.357481	37.252647
1723.027047	132705.623004	37.257664
1724.952305	132910.344856	37.262682
1726.136973	133111.186008	37.267700
1728.219924	133308.043597	37.272717
1729.876530	133516.324863	37.277735
1731.333497	133724.168700	37.282752
1733.475934	133931.970275	37.287770
1734.830109	134141.481628	37.292788
1736.782179	134352.766198	37.297805
1738.408163	134561.209420	37.302823
1740.074118	134766.069065	37.307840
1742.079612	134974.975408	37.312858
1743.833844	135194.821890	37.317876
1745.078355	135410.777030	37.322893
1747.406351	135617.364789	37.327911
1748.875482	135839.542881	37.332928
1750.977490	136042.779687	37.337946
1752.424700	136249.342459	37.342964
1754.162318	136448.704043	37.347981
1756.030904	136660.025146	37.352999
1757.908363	136869.163219	37.358016
1759.655417	137078.652478	37.363034
1761.575266	137278.560366	37.368052
1762.841646	137482.073236	37.373069
1764.866582	137679.758475	37.378087
1766.131571	137877.905469	37.383104
1767.653297	138078.437152	37.388122
1769.293680	138267.682431	37.393140
1770.348645	138480.509058	37.398157
1772.203865	138695.597868	37.403175
1773.817337	138908.123790	37.408192
1775.718236	139133.283579	37.413210
1777.318206	139348.719687	37.418228
1779.195639	139567.831899	37.423245
1781.148503	139780.182043	37.428263
1783.020650	140003.472277	37.433280
1784.850707	140212.632763	37.438298
1786.868293	140456.118652	37.443316
1788.896441	140682.839667	37.448333
1790.727347	140891.711118	37.453351
1791.942483	141120.908543	37.458368
1794.004593	141345.812620	37.463386
1796.027622	141561.789384	37.468404
1797.767834	141795.603962	37.473421
1799.337518	142015.486004	37.478439
1800.642059	142263.559291	37.483456
1802.448745	142498.242599	37.488474
1804.534003	142736.183412	37.493492
1806.259738	142979.270567	37.498509
1808.359315	143207.642169	37.503527
1810.132877	143453.935154	37.508544
1812.027385	143695.210080	37.513562
1813.808127	143932.823328	37.518580
1815.641065	144174.364002	37.523597
1817.374902	144414.398265	37.528615
1819.201788	144659.914737	37.533632
1820.925486	144907.352249	37.538650
1822.700106	145144.870680	37.543668
1824.411600	145409.878149	37.548685
1826.666722	145657.617393	37.553703
1828.401850	145918.143558	37.558720
1830.128526	146161.093741	37.563738
1832.077560	146416.689993	37.568756
1833.460998	146677.871304	37.573773
1835.563625	146932.253146	37.578791
1837.126507	147184.080227	37.583808
1839.084077	147451.230377	37.588826
1840.910690	147704.199340	37.593844
1842.727141	147973.646101	37.598861
1845.123685	148218.583294	37.603879
1847.375402	148471.908673	37.608896
1849.299509	148731.124938	37.613914
1851.282439	148975.000373	37.618932
1852.945665	149232.228845	37.623949
1855.278749	149474.465470	37.628967
1857.143119	149732.934355	37.633984
1859.036515	149988.188623	37.639002
1860.902432	150232.849613	37.644020
1862.441751	150487.793262	37.649037
1864.570973	150729.775344	37.654055
1865.840905	150981.564546	37.659072
1868.212244	151231.330265	37.664090
1870.199546	151481.106124	37.669108
1871.640531	151733.938426	37.674125
1873.599760	151971.319354	37.679143
1875.250465	152227.243895	37.684160
1877.054687	152479.109145	37.689178
1879.245712	152735.485076	37.694196
1880.960075	153000.568142	37.699213
1882.311016	153245.068852	37.704231
1884.327047	153491.637772	37.709248
1885.928942	153736.190420	37.714266
1887.633624	153966.383917	37.719284
1889.635811	154219.178229	37.724301
1891.472927	154466.820162	37.729319
1893.106899	154706.472077	37.734336
1894.715788	154963.519974	37.739354
1896.673300	155220.362433	37.744372
1898.403747	155478.206144	37.749389
1900.057532	155721.515173	37.754407
1901.462706	155992.068096	37.759424
1903.281364	156267.800750	37.764442
1905.740767	156534.891545	37.769460
1907.578732	156802.740392	37.774477
1909.665707	157071.554581	37.779495
1911.531616	157338.842945	37.784512
1913.390249	157619.856712	37.789530
1915.819432	157887.224907	37.794548
1917.386815	158160.352264	37.799565
1919.672118	158435.019475	37.804583
1921.849808	158694.470660	37.809600
1923.414594	158966.421432	37.814618
1925.421305	159241.592680	37.819636
1927.668335	159528.686635	37.824653
1929.329374	159806.364391	37.829671
1931.431597	160086.183719	37.834688
1932.849088	160373.169501	37.839706
1934.699971	160661.485654	37.844724
1936.407063	160949.927081	37.849741
1938.265701	161239.209545	37.854759
1940.254483	161536.750613	37.859776
1941.914803	161841.568031	37.864794
1944.144805	162131.609299	37.869812
1946.078433	162440.297326	37.874829
1948.576897	162728.395150	37.879847
1950.893891	163019.886916	37.884864
1952.858571	163318.849262	37.889882
1954.679836	163616.299083	37.894900
1956.303173	163919.798998	37.899917
1958.471820	164216.334145	37.904935
1960.748210	164509.844860	37.909952
1963.192661	164801.883346	37.914970
1965.609255	165077.168343	37.919988
1967.559420	165370.505086	37.925005
1969.580119	165655.795309	37.930023
1972.023173	165950.429076	37.935040
1973.562161	166234.692114	37.940058
1975.500363	166514.996361	37.945076
1977.389995	166801.378292	37.950093
1979.266355	167091.458208	37.955111
1981.314214	167392.634974	37.960128
1983.003156	167673.782606	37.965146
1985.073312	167963.264639	37.970164
1987.076166	168262.179420	37.975181
1989.101176	168542.732258	37.980199
1991.098897	168836.888915	37.985216
1993.082635	169125.805086	37.990234
1994.800871	169413.786065	37.995252
1996.723868	169709.837098	38.000269
1998.522855	169999.610836	38.005287
2000.897544	170313.852584	38.010304
2002.416769	170610.071690	38.015322
2004.703487	170898.262096	38.020340
2006.616908	171209.354327	38.025357
2008.568194	171508.671433	38.030375
2010.305990	171815.692248	38.035392
2012.146144	172115.384596	38.040410
2014.106768	172426.804658	38.045428
2016.171337	172734.210056	38.050445
2017.960337	173021.025815	38.055463
2019.883603	173316.595886	38.060480
2021.389862	173614.454099	38.065498
2023.529341	173894.425226	38.070516
2025.564632	174205.320224	38.075533
2027.389076	174499.170537	38.080551
2029.442669	174802.916099	38.085568
2031.401075	175120.442301	38.090586
2033.365227	175418.743967	38.095604
2035.014440	175735.838189	38.100621
2037.290675	176037.166511	38.105639
2039.585774	176350.492832	38.110656
2041.362054	176680.485040	38.115674
2043.552914	176996.801435	38.120692
2045.576198	177318.770490	38.125709
2047.750204	177636.501448	38.130727
2049.535676	177956.909954	38.135744
2051.550362	178286.706296	38.140762
2053.290007	178613.753029	38.145780
2055.140320	178952.314122	38.150797
2057.642237	179296.057772	38.155815
2059.892450	179616.298527	38.160832
2062.055181	179960.808697	38.165850
2064.171507	180286.736368	38.170868
2066.334097	180634.652448	38.175885
2068.716292	180965.442967	38.180903
2070.745251	181294.334029	38.185920
2072.646918	181632.059189	38.190938
2074.889667	181969.757902	38.195956
2077.282723	182310.583828	38.200973
2079.295056	182647.000152	38.205991
2081.819935	182981.763211	38.211008
2083.409041	183327.518224	38.216026
2085.322148	183666.823628	38.221044
2087.580989	184022.331544	38.226061
2089.888052	184363.533770	38.231079
2091.999180	184694.023980	38.236096
2094.378718	185036.411001	38.241114
2096.807460	185402.717388	38.246132
2099.021334	185784.501191	38.251149
2100.978461	186132.875669	38.256167
2103.446140	186466.414906	38.261184
2104.991145	186808.734590	38.266202
2107.243915	187142.309445	38.271220
2109.055613	187478.849546	38.276237
2111.075565	187830.115460	38.281255
2113.130458	188169.439246	38.286272
2115.182309	188539.523665	38.291290
2116.906609	188876.462735	38.296308
2119.499249	189237.905608	38.301325
2121.948161	189573.616434	38.306343
2124.379417	189922.234245	38.311360
2125.905452	190280.392062	38.316378
2128.115737	190627.725616	38.321396
2130.495902	190972.823949	38.326413
2132.497292	191327.558193	38.331431
2134.783788	191670.844331	38.336448
2136.278608	192036.302322	38.341466
2138.620935	192375.187500	38.346484
2141.043933	192730.393698	38.351501
2142.864706	193090.088976	38.356519
2145.113159	193434.960861	38.361536
2147.155984	193800.491215	38.366554
2148.978917	194164.202573	38.371572
2150.940188	194521.365366	38.376589
2153.120489	194888.223675	38.381607
2155.846363	195240.925852	38.386624
2157.697025	195592.571316	38.391642
2159.831493	195933.708195	38.396660
2161.591863	196282.346749	38.401677
2163.573206	196617.362033	38.406695
2165.876306	196959.770684	38.411712
2167.268197	197319.417222	38.416730
2169.548913	197678.164292	38.421748
2171.741909	198026.130191	38.426765
2173.900258	198388.124071	38.431783
2175.339055	198740.527330	38.436800
2177.643871	199123.456685	38.441818
2179.736374	199491.509115	38.446836
2181.918993	199873.443285	38.451853
2183.726251	200255.817833	38.456871
2185.890932	200643.903955	38.461888
2187.614896	201035.184065	38.466906
2189.721425	201435.499570	38.471924
2192.289170	201823.297136	38.476941
2194.203123	202225.041619	38.481959
2196.918190	202621.327858	38.486976
2199.285641	203031.259413	38.491994
2201.959549	203428.747786	38.497012
2204.209344	203821.679765	38.502029
2206.574092	204232.884586	38.507047
2208.810749	204632.323393	38.512064
2210.874206	205038.013659	38.517082
2212.833767	205448.801496	38.522100
2215.233667	205853.043924	38.527117
2217.519974	206260.175362	38.532135
2219.555796	206662.545426	38.537152
2221.476003	207089.981597	38.542170
2223.505213	207503.938035	38.547188
2225.465097	207927.330581	38.552205
2227.763776	208351.484093	38.557223
2230.630552	208776.947144	38.562240
2233.169053	209198.016479	38.567258
2235.163071	209618.637810	38.572276
2237.283185	210036.572875	38.577293
2239.510620	210458.683472	38.582311
2242.510381	210878.388244	38.587328
2244.805956	211301.404090	38.592346
2247.335317	211719.963989	38.597364
2249.735439	212138.519208	38.602381
2252.047041	212562.957014	38.607399
2254.494930	212981.226534	38.612416
2256.694847	213397.401298	38.617434
2259.003137	213813.940782	38.622452
2261.270092	214221.976984	38.627469
2263.102149	214645.018722	38.632487
2265.400681	215066.972210	38.637504
2267.344564	215507.297475	38.642522
2269.613859	215929.459692	38.647540
2272.471658	216351.276721	38.652557
2274.344639	216782.214987	38.657575
2276.492871	217207.115521	38.662592
2278.786561	217644.721149	38.667610
2281.106275	218077.470971	38.672628
2283.403984	218503.263902	38.677645
2285.469857	218959.908229	38.682663
2287.687890	219381.700396	38.687680
2289.704125	219814.473370	38.692698
2292.323271	220253.656219	38.697716
2294.842943	220676.494633	38.702733
2296.774612	221122.440834	38.707751
2299.543202	221558.755912	38.712768
2301.500700	221993.368330	38.717786
2304.186771	222423.167794	38.722804
2306.217439	222853.831536	38.727821
2308.677069	223276.477185	38.732839
2311.329633	223686.136843	38.737856
2313.915616	224086.305826	38.742874
2315.905132	224491.369081	38.747892
2318.846421	224876.113422	38.752909
2320.611752	225285.022279	38.757927
2323.487955	225674.654400	38.762944
2325.444804	226080.383380	38.767962
2327.763901	226467.129926	38.772980
2330.274613	226875.999004	38.777997
2332.852190	227263.670624	38.783015
2335.328309	227651.459601	38.788032
2337.538703	228063.804810	38.793050
2339.635468	228462.525624	38.798068
2341.943344	228863.855509	38.803085
2344.178464	229289.635310	38.808103
2346.233513	229709.218993	38.813120
2348.149785	230121.329917	38.818138
2349.957530	230548.954016	38.823156
2352.860154	230974.476813	38.828173
2354.915177	231409.022696	38.833191
2357.326164	231853.268060	38.838208
2359.222269	232303.359970	38.843226
2361.629342	232743.870965	38.848244
2364.387845	233177.671114	38.853261
2366.469179	233642.492878	38.858279
2368.521183	234096.369721	38.863296
2370.700669	234548.422638	38.868314
2373.069792	235011.928150	38.873332
2375.202276	235479.356794	38.878349
2377.819416	235947.954289	38.883367
2380.267239	236419.956295	38.888384
2382.323596	236904.390264	38.893402
2384.693837	237376.352350	38.898420
2387.049741	237860.179551	38.903437
2389.536320	238347.948697	38.908455
2391.667242	238835.340607	38.913472
2394.245239	239333.814346	38.918490
2396.713042	239817.799021	38.923508
2399.499257	240304.984989	38.928525
2401.669700	240798.820031	38.933543
2404.561863	241286.292640	38.938560
2406.895668	241781.091195	38.943578
2409.370904	242265.705483	38.948596
2411.969003	242752.611404	38.953613
2414.209760	243245.897348	38.958631
2416.490908	243738.515493	38.963648
2418.957631	244230.900477	38.968666
2421.188618	244739.578980	38.973684
2423.639343	245230.770276	38.978701
2426.426118	245726.760084	38.983719
2428.797087	246227.004874	38.988736
2431.317822	246712.542320	38.993754
2433.382172	247208.158252	38.998772
2436.383751	247705.456039	39.003789
2438.295862	248225.657340	39.008807
2440.902098	248730.025006	39.013824
2443.859705	249226.360213	39.018842
2446.583166	249728.852417	39.023860
2448.852456	250222.218209	39.028877
2451.104875	250732.071199	39.033895
2453.177613	251217.437537	39.038912
2456.029073	251726.940171	39.043930
2458.294175	252234.119230	39.048948
2461.134155	252720.428441	39.053965
2463.753328	253219.064927	39.058983
2466.034434	253716.075851	39.064000
2468.779866	254215.121167	39.069018
2470.775392	254708.591520	39.074036
2473.555782	255184.614233	39.079053
2475.757613	255655.162464	39.084071
2478.144418	256131.547989	39.089088
2480.773719	256593.110613	39.094106
2482.929182	257065.667844	39.099124
2485.670161	257539.503907	39.104141
2489.039355	257989.008007	39.109159
2491.475203	258449.044701	39.114176
2494.172021	258919.681997	39.119194
2496.413050	259379.008956	39.124212
2499.011724	259847.803725	39.129229
2501.524148	260324.662025	39.134247
2503.750777	260800.851677	39.139264
2505.805024	261275.516805	39.144282
2507.508120	261760.699474	39.149300
2510.030955	262244.685709	39.154317
2512.803999	262746.995042	39.159335
2515.465063	263243.883974	39.164352
2517.709710	263745.000995	39.169370
2520.080922	264244.165631	39.174388
2522.834216	264753.377435	39.179405
2525.650186	265252.493500	39.184423
2527.844512	265765.317860	39.189440
2530.677362	266274.128834	39.194458
2532.989249	266790.968182	39.199476
2535.091006	267306.389826	39.204493
2537.847450	267830.545623	39.209511
2540.429065	268345.912525	39.214528
2542.630695	268870.479213	39.219546
2545.193637	269423.331196	39.224564
2547.753265	269947.379024	39.229581
2550.373766	270490.920027	39.234599
2552.983223	271023.716265	39.239616
2555.467517	271569.608621	39.244634
2557.968529	272111.583834	39.249652
2560.577912	272653.411873	39.254669
2563.149417	273213.909351	39.259687
2565.086504	273760.584372	39.264704
2567.943758	274310.973011	39.269722
2570.508612	274871.130482	39.274740
2573.634428	275416.390742	39.279757
2575.893629	275980.829496	39.284775
2578.890595	276540.578228	39.289792
2581.262803	277098.287038	39.294810
2583.893201	277659.405596	39.299828
2586.960991	278214.636503	39.304845
2588.930447	278780.268737	39.309863
2591.688130	279346.916950	39.314880
2594.351170	279903.697017	39.319898
2597.393757	280475.041354	39.324916
2600.326501	281033.142409	39.329933
2602.894530	281590.483392	39.334951
2605.511971	282140.905206	39.339968
2608.419930	282697.727732	39.344986
2610.997723	283252.235694	39.350004
2613.740823	283799.349442	39.355021
2616.716380	284358.992546	39.360039
2618.881671	284911.367813	39.365056
2622.024999	285456.197080	39.370074
2624.400152	286005.712278	39.375092
2627.279919	286550.218323	39.380109
2630.084163	287089.907146	39.385127
2632.646432	287635.367910	39.390144
2635.891528	288172.084614	39.395162
2638.300705	288711.974029	39.400180
2640.708768	289243.759200	39.405197
2643.532877	289787.459989	39.410215
2646.204508	290325.136772	39.415232
2648.810073	290831.258264	39.420250
2650.842990	291338.099564	39.425268
2653.808666	291844.207607	39.430285
2655.921693	292365.983111	39.435303
2657.839854	292895.401555	39.440320
2660.536893	293405.220105	39.445338
2662.910305	293935.853513	39.450356
2665.219950	294471.900112	39.455373
2667.236300	295017.457720	39.460391
2670.023809	295571.065545	39.465408
2672.832336	296127.787686	39.470426
2675.131213	296690.829382	39.475444
2677.707006	297247.805462	39.480461
2680.150418	297820.892731	39.485479
2682.022042	298405.792343	39.490496
2684.818917	298993.131416	39.495514
2687.571531	299585.878676	39.500532
2690.298102	300179.664508	39.505549
2692.784583	300777.035418	39.510567
2695.282578	301381.785431	39.515584
2698.607695	301992.111835	39.520602
2701.048213	302620.973667	39.525620
2703.745742	303227.321885	39.530637
2706.020298	303851.955547	39.535655
2708.753472	304480.775051	39.540672
2711.852091	305103.412376	39.545690
2714.298989	305740.688795	39.550708
2717.110683	306371.351429	39.555725
2720.026869	307013.285684	39.560743
2722.607823	307641.861510	39.565760
2725.869273	308271.313458	39.570778
2728.984561	308919.284126	39.575796
2732.318843	309543.733490	39.580813
2735.202488	310176.697197	39.585831
2737.573059	310813.844302	39.590848
2740.527111	311435.333380	39.595866
2743.341765	312075.643390	39.600884
2746.288467	312704.223691	39.605901
2749.780978	313334.487266	39.610919
2752.040109	313963.436836	39.615936
2754.790413	314594.966291	39.620954
2757.724746	315222.651536	39.625972
2760.866603	315846.336736	39.630989
2763.763856	316471.218832	39.636007
2766.874946	317095.957463	39.641024
2770.020156	317711.520628	39.646042
2772.841837	318325.704462	39.651060
2775.730570	318947.203315	39.656077
2778.743155	319555.198977	39.661095
2781.457834	320175.565472	39.666112
2784.745898	320773.858119	39.671130
2787.156404	321389.712143	39.676148
2790.318433	321994.021403	39.681165
2793.061760	322595.595954	39.686183
2795.344413	323215.046623	39.691200
2798.414332	323810.488406	39.696218
2801.280305	324426.303299	39.701236
2804.163548	325038.021192	39.706253
2806.965244	325649.894908	39.711271
2809.364339	326268.368289	39.716288
2812.034934	326878.975298	39.721306
2814.818019	327485.825874	39.726324
2817.672065	328101.739268	39.731341
2820.752988	328716.694473	39.736359
2823.532560	329323.035568	39.741376
2826.334414	329929.998123	39.746394
2828.951828	330542.536012	39.751412
2831.429659	331148.109328	39.756429
2834.135130	331736.462748	39.761447
2836.811150	332331.762829	39.766464
2839.745894	332910.143339	39.771482
2842.054281	333498.429987	39.776500
2844.637140	334091.205599	39.781517
2847.238915	334681.787344	39.786535
2849.623305	335302.148969	39.791552
2852.252286	335911.326314	39.796570
2854.901378	336529.799843	39.801588
2857.550746	337157.343827	39.806605
2860.604767	337784.966269	39.811623
2863.049287	338431.163621	39.816640
2865.931622	339064.041150	39.821658
2868.280110	339714.212658	39.826676
2871.195653	340370.193768	39.831693
2874.160020	341020.575344	39.836711
2877.144123	341681.898448	39.841728
2880.315728	342355.226849	39.846746
2883.032424	343017.175058	39.851764
2885.684700	343683.989988	39.856781
2888.957869	344368.777437	39.861799
2891.299031	345049.841556	39.866816
2894.610408	345727.824779	39.871834
2897.315344	346412.000339	39.876852
2900.528454	347101.940751	39.881869
2903.879378	347797.474986	39.886887
2906.225415	348492.618596	39.891904
2909.633869	349167.880061	39.896922
2912.626725	349861.474281	39.901940
2915.914008	350556.326524	39.906957
2919.415521	351237.590937	39.911975
2922.520030	351926.864201	39.916992
2925.667583	352616.927376	39.922010
2928.821200	353300.180003	39.927028
2931.358983	353987.367504	39.932045
2934.391413	354666.755993	39.937063
2937.407555	355357.997123	39.942080
2940.593725	356041.641860	39.947098
2943.524147	356729.240818	39.952116
2946.026835	357418.488193	39.957133
2948.832991	358114.416005	39.962151
2951.908461	358813.328055	39.967168
2954.917803	359523.970806	39.972186
2957.788819	360222.375415	39.977204
2960.556819	360934.239395	39.982221
2963.970788	361628.293966	39.987239
2967.026935	362325.581750	39.992256
2969.737453	363027.722662	39.997274
2972.753890	363728.253289	40.002292
2975.998352	364436.309759	40.007309
2978.920556	365126.760012	40.012327
2982.009862	365842.435073	40.017344
2984.756836	366542.433386	40.022362
2988.249675	367241.107597	40.027380
2991.130967	367958.232441	40.032397
2994.353414	368643.280929	40.037415
2997.644180	369347.180649	40.042432
3000.645276	370045.482591	40.047450
3003.624659	370738.702841	40.052468
3006.745827	371429.704804	40.057485
3010.386713	372112.652782	40.062503
3013.329729	372808.614400	40.067520
3016.339091	373491.778674	40.072538
3019.447756	374165.688340	40.077556
3022.688801	374870.976278	40.082573
3025.321645	375544.393940	40.087591
3028.540926	376232.650552	40.092608
3031.327782	376902.945059	40.097626
3034.192435	377560.113841	40.102644
3036.530271	378219.628336	40.107661
3039.767056	378874.148349	40.112679
3042.274002	379529.855002	40.117696
3045.168839	380194.730471	40.122714
3048.568500	380856.344402	40.127732
3051.219690	381528.569502	40.132749
3054.182997	382192.243801	40.137767
3056.893042	382864.146624	40.142784
3059.654480	383547.091770	40.147802
3062.807712	384236.694555	40.152820
3065.580517	384942.242305	40.157837
3068.771506	385628.610665	40.162855
3071.459597	386342.262003	40.167872
3074.259462	387050.405980	40.172890
3077.247550	387764.274280	40.177908
3079.861022	388485.878364	40.182925
3083.052632	389221.880574	40.187943
3086.059798	389963.890576	40.192960
3089.393654	390696.990943	40.197978
3092.531066	391452.279278	40.202996
3095.532023	392210.502436	40.208013
3098.366011	392958.854285	40.213031
3101.331225	393722.757542	40.218048
3104.555734	394479.710444	40.223066
3108.136272	395247.317584	40.228084
3110.906631	396009.558350	40.233101
3113.946152	396781.604981	40.238119
3117.246232	397556.370286	40.243136
3120.386711	398330.831256	40.248154
3123.768946	399105.684668	40.253172
3126.617286	399895.730762	40.258189
3129.545945	400682.447386	40.263207
3132.881830	401465.227102	40.268224
3136.196716	402259.726079	40.273242
3139.306477	403052.862942	40.278260
3142.192653	403854.610938	40.283277
3145.448854	404647.821378	40.288295
3148.563501	405447.149558	40.293312
3151.492130	406263.330001	40.298330
3155.022104	407066.179620	40.303348
3158.135378	407870.330278	40.308365
3161.421787	408673.210520	40.313383
3164.712648	409508.140211	40.318400
3167.813017	410309.775566	40.323418
3171.152596	411122.222218	40.328436
3174.237565	411947.933517	40.333453
3177.914328	412747.416607	40.338471
3181.481251	413553.868514	40.343488
3184.535909	414364.973365	40.348506
3188.341280	415156.152016	40.353524
3191.411946	415965.018616	40.358541
3194.818652	416772.689388	40.363559
3197.960720	417577.133476	40.368576
3200.684193	418382.117797	40.373594
3204.322942	419190.064514	40.378612
3207.547275	420004.973056	40.383629
3211.037561	420802.512898	40.388647
3214.530962	421607.859847	40.393664
3217.029958	422410.447780	40.398682
3220.202007	423215.680763	40.403700
3223.730626	424020.472652	40.408717
3227.063131	424831.785729	40.413735
3230.595876	425626.856189	40.418752
3233.953191	426430.517468	40.423770
3237.731921	427208.398892	40.428788
3241.101135	428007.647480	40.433805
3244.613085	428772.719578	40.438823
3247.710908	429534.439879	40.443840
3250.544584	430277.014423	40.448858
3253.954783	431024.323742	40.453876
3256.757314	431770.284009	40.458893
3259.853012	432524.509709	40.463911
3262.992492	433273.847628	40.468928
3266.113121	434031.447875	40.473946
3269.591473	434797.756131	40.478964
3272.513068	435575.541317	40.483981
3275.200229	436345.953876	40.488999
3278.510446	437130.740622	40.494016
3281.616607	437937.809648	40.499034
3284.895185	438729.609372	40.504052
3287.953146	439528.988878	40.509069
3290.934150	440343.300848	40.514087
3294.008324	441166.100800	40.519104
3296.972718	441988.629109	40.524122
3300.294359	442807.883138	40.529140
3303.237022	443657.568527	40.534157
3306.475740	444502.067327	40.539175
3310.565528	445351.142741	40.544192
3313.907094	446204.083225	40.549210
3317.378084	447059.993978	40.554228
3320.157260	447925.971305	40.559245
3323.777725	448787.484045	40.564263
3328.074504	449654.606994	40.569280
3331.436977	450529.861998	40.574298
3335.102161	451388.466141	40.579316
3338.323363	452257.852140	40.584333
3341.756953	453131.251966	40.589351
3345.231780	453996.222052	40.594368
3348.757422	454881.435211	40.599386
3352.564903	455749.195332	40.604404
3355.767114	456629.373244	40.609421
3359.208585	457512.901699	40.614439
3363.247952	458381.706100	40.619456
3366.419218	459265.893859	40.624474
3369.943493	460154.674645	40.629492
3373.177921	461044.968419	40.634509
3377.016787	461922.304837	40.639527
3380.299003	462805.989924	40.644544
3383.406818	463694.197109	40.649562
3386.757778	464584.136091	40.654580
3390.103170	465477.509955	40.659597
3393.138674	466375.878740	40.664615
3396.375770	467277.345867	40.669632
3399.952703	468193.339388	40.674650
3403.874520	469090.314052	40.679668
3407.537555	470004.882491	40.684685
3411.011813	470900.516962	40.689703
3414.544592	471798.413200	40.694720
3418.335837	472693.597599	40.699738
3422.062338	473590.558113	40.704756
3425.729407	474491.713703	40.709773
3429.028767	475383.800715	40.714791
3432.476168	476276.571474	40.719808
3435.728259	477174.717180	40.724826
3439.571714	478069.897334	40.729844
3442.915567	478974.430366	40.734861
3446.204355	479870.905913	40.739879
3450.116498	480750.953582	40.744896
3453.485863	481649.230753	40.749914
3457.253980	482545.328145	40.754932
3460.308968	483437.503990	40.759949
3464.068842	484318.181052	40.764967
3467.605256	485206.552256	40.769984
3471.186554	486098.392374	40.775002
3475.000177	486965.598463	40.780007
3478.469162	487795.035852	40.785012
3481.391352	488578.906623	40.790016
3485.161883	489303.617160	40.795021
3488.311322	489980.413718	40.800026
3491.562795	490598.938777	40.805031
3494.231331	491162.083350	40.810036
3496.233894	491673.603179	40.815040
3499.089677	492115.392193	40.820045
3501.094810	492531.145405	40.825050
3502.972651	492883.085795	40.830055
3505.598328	493180.674859	40.835060
3507.138262	493459.947790	40.840064
3508.694458	493664.843073	40.845069
3509.797213	493861.425067	40.850074
3511.382108	493989.771126	40.855079
3512.340312	494098.574016	40.860084
3513.600742	494174.411507	40.865088
3515.034804	494214.476840	40.870093
3515.739418	494230.219914	40.875098
3516.584395	494209.540037	40.880103
3517.610600	494178.027690	40.885108
3518.112338	494111.811152	40.890112
3518.710825	494038.813930	40.895117
3519.089242	493937.425920	40.900122
3519.795061	493812.054814	40.905127
3520.269218	493684.093291	40.910132
3520.612068	493529.947182	40.915136
3520.836250	493363.599410	40.920141
3521.556029	493193.739321	40.925146
3521.990765	492999.786944	40.930151
3522.160821	492798.602437	40.935156
3522.144151	492582.599505	40.940160
3522.164923	492353.661372	40.945165
3522.157916	492120.078626	40.950170
3522.121840	491896.646236	40.955175
3522.375206	491670.186255	40.960180
3522.391999	491430.883124	40.965184
3522.594444	491175.388211	40.970189
3522.320444	490926.982349	40.975194
3522.098419	490666.242589	40.980199
3521.946025	490421.546423	40.985204
3521.703341	490160.245669	40.990208
3522.012577	489894.460900	40.995213
3521.847792	489643.138411	41.000218
3521.948531	489366.821871	41.005223
3521.363473	489105.354237	41.010228
3521.185306	488848.515757	41.015232
3521.309500	488583.746992	41.020237
3521.409051	488330.745528	41.025242
3521.232390	488065.661052	41.030247
3521.055362	487805.673388	41.035252
3520.814952	487539.832097	41.040256
3521.225588	487268.429787	41.045261
3520.299570	487014.454941	41.050266
3520.660155	486748.051809	41.055271
3519.988331	486492.614446	41.060276
3519.704097	486226.302621	41.065280
3519.879570	485965.420732	41.070285
3519.618882	485719.201219	41.075290
3519.159332	485466.744731	41.080295
3519.587925	485211.771617	41.085300
3519.035092	484968.768172	41.090304
3519.067127	484705.967673	41.095309
3518.258315	484463.652877	41.100314
3518.059985	484214.873757	41.105319
3518.457615	483979.941693	41.110324
3517.714618	483744.728882	41.115328
3517.866699	483508.817481	41.120333
3517.612454	483275.896083	41.125338
3517.340569	483038.123649	41.130343
3517.637773	482798.136995	41.135348
3517.184136	482581.858901	41.140352
3517.113762	482340.659285	41.145357
3516.806788	482126.827860	41.150362
3516.624738	481896.097843	41.155367
3516.357212	481675.786581	41.160372
3515.812037	481464.610663	41.165376
3515.902795	481237.921367	41.170381
3515.445316	481030.212517	41.175386
3515.322583	480825.682824	41.180391
3515.402075	480618.036568	41.185396
3515.009034	480419.304283	41.190400
3515.193888	480206.835636	41.195405
3514.621300	480009.490521	41.200410
3514.933936	479807.558163	41.205415
3514.563786	479614.522569	41.210420
3514.408174	479411.192503	41.215424
3514.613571	479216.091597	41.220429
3514.252468	479024.159195	41.225434
3513.988916	478826.448015	41.230439
3513.817246	478643.022358	41.235444
3513.757125	478455.483592	41.240448
3513.896587	478271.853620	41.245453
3513.196741	478102.200048	41.250458
3513.019281	477909.416964	41.255463
3513.278295	477730.967813	41.260468
3512.610231	477555.339632	41.265472
3512.839347	477376.486837	41.270477
3512.722992	477216.790915	41.275482
3512.482380	477036.895477	41.280487
3512.622642	476879.582326	41.285492
3512.119010	476704.879536	41.290496
3512.119828	476541.165642	41.295501
3511.844727	476384.013349	41.300506
3511.941003	476216.086026	41.305511
3511.428135	476067.712047	41.310516
3511.310532	475914.877625	41.315520
3511.238836	475754.856902	41.320525
3510.857207	475599.634300	41.325530
3510.962244	475456.061645	41.330535
3511.115472	475312.075823	41.335540
3510.604160	475164.956983	41.340544
3510.638633	475018.560662	41.345549
3510.611305	474874.497928	41.350554
3510.728382	474727.782815	41.355559
3510.809774	474599.219683	41.360564
3510.020648	474458.102626	41.365568
3510.448446	474318.968690	41.370573
3509.929268	474182.356870	41.375578
3509.846126	474054.826057	41.380583
3510.433266	473923.297358	41.385588
3510.024302	473786.108961	41.390592
3509.953091	473647.805213	41.395597
3509.660508	473514.286833	41.400602
3509.781812	473386.162848	41.405607
3509.738000	473260.237413	41.410612
3509.100065	473136.931224	41.415616
3509.521785	473001.224699	41.420621
3509.152814	472881.767518	41.425626
3509.271282	472758.441865	41.430631
3509.133491	472634.649586	41.435636
3508.879713	472528.215576	41.440640
3509.287532	472393.264508	41.445645
3509.268903	472285.022798	41.450650
3509.150079	472151.213399	41.455655
3508.943298	472045.881213	41.460660
3508.494727	471925.974382	41.465664
3508.703483	471803.537524	41.470669
3508.699259	471696.149181	41.475674
3508.855357	471580.443309	41.480679
3507.893338	471471.938531	41.485684
3508.203052	471360.454286	41.490688
3508.435249	471253.076806	41.495693
3507.957849	471151.573062	41.500698
3508.029129	471044.977683	41.505703
3508.188183	470936.446588	41.510708
3507.878272	470841.083447	41.515712
3507.914312	470736.918550	41.520717
3507.468376	470638.794445	41.525722
3507.844636	470534.676450	41.530727
3507.525577	470434.053768	41.535732
3507.348456	470333.964587	41.540736
3507.739516	470229.033329	41.545741
3507.535128	470137.239752	41.550746
3507.496019	470044.661470	41.555751
3507.646611	469946.946058	41.560756
3507.550076	469854.931863	41.565760
3507.407015	469752.153871	41.570765
3507.437408	469657.539964	41.575770
3507.412638	469557.220090	41.580775
3507.303537	469469.402715	41.585780
3507.480532	469374.713807	41.590784
3507.342537	469269.656505	41.595789
3507.075568	469181.761031	41.600794
3506.937738	469081.607564	41.605799
3506.808837	468998.493581	41.610804
3506.979341	468903.701849	41.615808
3507.201195	468819.622154	41.620813
3506.877960	468736.081975	41.625818
3506.839455	468644.911682	41.630823
3506.792581	468553.034216	41.635828
3506.731355	468474.154909	41.640832
3506.681851	468384.046857	41.645837
3506.604263	468296.016069	41.650842
3506.735470	468213.515085	41.655847
3506.671432	468132.409486	41.660852
3505.817243	468055.168704	41.665856
3506.154581	467972.179305	41.670861
3506.094426	467902.501087	41.675866
3506.297776	467817.913480	41.680871
3506.521807	467739.947158	41.685876
3506.029090	467656.883064	41.690880
3506.635492	467585.380337	41.695885
3506.725940	467501.516705	41.700890
3506.746534	467413.415390	41.705895
3506.446178	467334.719604	41.710900
3506.318831	467256.350538	41.715904
3506.376347	467171.175457	41.720909
3506.311623	467087.081018	41.725914
3506.379464	467013.535538	41.730919
3506.268291	466928.992361	41.735924
3506.046902	466851.141769	41.740928
3506.464636	466774.860330	41.745933
3506.121512	466690.099163	41.750938
3506.049708	466616.674816	41.755943
3506.021585	466540.512264	41.760948
3505.917412	466458.544974	41.765952
3506.162074	466390.785463	41.770957
3506.210217	466321.741274	41.775962
3506.477293	466234.455179	41.780967
3505.951205	466163.173172	41.785972
3506.034190	466086.384341	41.790976
3505.900075	466018.935153	41.795981
3506.025989	465934.805250	41.800986
3505.747520	465848.107810	41.805991
3505.788943	465779.416476	41.810996
3505.347089	465713.278393	41.816000
3505.537887	465648.558951	41.821005
3505.263420	465579.157278	41.826010
3505.277386	465513.908470	41.831015
3505.355497	465454.718898	41.836020
3505.459542	465394.260604	41.841024
3505.394999	465320.273075	41.846029
3505.527956	465255.207063	41.851034
3505.424316	465193.111240	41.856039
3505.489695	465122.744362	41.861044
3505.483532	465059.368378	41.866048
3505.390256	464989.632593	41.871053
3505.423771	464927.160383	41.876058
3505.696866	464862.728593	41.881063
3505.657948	464797.687558	41.886068
3505.262957	464732.044127	41.891072
3505.359936	464663.036100	41.896077
3505.533488	464601.400772	41.901082
3505.502082	464528.315071	41.906087
3505.366739	464453.727769	41.911092
3505.110344	464395.294672	41.916096
3505.128435	464321.795716	41.921101
3505.229201	464258.298916	41.926106
3505.084551	464205.816509	41.931111
3505.220581	464146.815658	41.936116
3505.327365	464088.729647	41.941120
3505.696572	464018.766129	41.946125
3505.448340	463960.583173	41.951130
3505.272088	463884.937473	41.956135
3505.329244	463823.165667	41.961140
3505.468000	463761.330353	41.966144
3505.404916	463682.681682	41.971149
3505.053159	463626.537054	41.976154
3505.086973	463569.573473	41.981159
3505.498843	463498.033042	41.986164
3505.246946	463436.712597	41.991168
3505.266087	463369.835970	41.996173
3504.917720	463310.401730	42.001178
3505.280851	463251.716517	42.006183
3505.377781	463182.803627	42.011188
3505.220763	463115.801654	42.016192
3505.217942	463049.230696	42.021197
3504.982692	462990.384764	42.026202
3504.958052	462936.918607	42.031207
3505.268710	462868.021767	42.036212
3504.600670	462816.324711	42.041216
3504.935977	462756.579794	42.046221
3505.041093	462701.828031	42.051226
3504.997919	462636.577001	42.056231
3504.980450	462574.002860	42.061236
3504.848347	462520.855642	42.066240
3504.907725	462450.276229	42.071245
3504.823164	462396.261229	42.076250
3504.687484	462338.055188	42.081255
3504.741638	462283.158243	42.086260
3504.698139	462236.876371	42.091264
3504.977320	462168.993370	42.096269
3504.733019	462114.294090	42.101274
3504.764149	462054.846990	42.106279
3504.761784	461997.833179	42.111284
3504.286584	461956.524880	42.116288
3504.609955	461896.222321	42.121293
3504.840862	461855.967459	42.126298
3504.714440	461786.223643	42.131303
3504.613500	461734.435048	42.136308
3504.411942	461685.849134	42.141312
3504.807963	461618.957567	42.146317
3504.565345	461559.146615	42.151322
3504.630872	461515.527119	42.156327
3504.827573	461460.807708	42.161332
3504.613012	461409.440535	42.166336
3504.461938	461358.468056	42.171341
3504.412190	461302.875850	42.176346
3504.749406	461251.523521	42.181351
3504.552719	461191.451178	42.186356
3504.418779	461139.362364	42.191360
3504.434118	461078.345977	42.196365
3504.134600	461034.630283	42.201370
3504.454816	460981.509067	42.206375
3504.375106	460937.860106	42.211380
3504.332975	460888.842379	42.216384
3504.427764	460835.553419	42.221389
3504.094871	460796.648616	42.226394
3504.522355	460740.980322	42.231399
3504.761559	460691.108762	42.236404
3504.219028	460638.778449	42.241408
3504.293340	460578.459410	42.246413
3504.069802	460538.069793	42.251418
3503.775799	460490.304366	42.256423
3504.505680	460443.998480	42.261428
3504.237838	460397.999509	42.266432
3504.463136	460337.554941	42.271437
3504.436227	460299.967438	42.276442
3504.241735	460248.593659	42.281447
3504.645004	460204.715892	42.286452
3504.244494	460150.995936	42.291456
3504.294335	460088.149248	42.296461
3504.068280	460054.538599	42.301466
3504.205984	459999.165971	42.306471
3504.236231	459948.464654	42.311476
3504.293947	459899.529755	42.316480
3504.564474	459837.609124	42.321485
3504.392499	459798.778208	42.326490
3504.482036	459746.397411	42.331495
3504.279833	459689.508207	42.336500
3504.251625	459642.306214	42.341504
3504.451514	459588.187492	42.346509
3504.111544	459545.992192	42.351514
3504.158241	459495.539965	42.356519
3504.574787	459449.533150	42.361524
3504.323160	459410.359576	42.366528
3503.812447	459353.719658	42.371533
3503.843604	459308.177215	42.376538
3504.063031	459266.450749	42.381543
3504.129443	459209.720551	42.386548
3504.398436	459170.060636	42.391552
3504.261245	459111.388491	42.396557
3503.780729	459068.505523	42.401562
3503.878002	459028.568418	42.406567
3503.905010	458987.832584	42.411572
3503.794918	458947.370981	42.416576
3504.377346	458888.889688	42.421581
3503.813290	458847.334729	42.426586
3503.981950	458814.672208	42.431591
3504.088801	458772.152490	42.436596
3503.999335	458720.100025	42.441600
3503.912755	458677.104184	42.446605
3504.171929	458642.251495	42.451610
3504.131466	458589.027230	42.456615
3504.547961	458543.119212	42.461620
3504.331195	458487.442698	42.466624
3504.324427	458438.361892	42.471629
3504.286587	458389.488182	42.476634
3504.290504	458341.721037	42.481639
3504.352244	458288.226944	42.486644
3504.096367	458242.726360	42.491648
3504.216113	458187.502519	42.496653
3504.029451	458139.663272	42.501658
3503.890846	458102.138963	42.506663
3503.997543	458048.586534	42.511668
3503.921832	458007.408971	42.516672
3504.037907	457966.505072	42.521677
3504.179767	457914.161183	42.526682
3504.147325	457873.684986	42.531687
3503.966745	457825.894529	42.536692
3503.575607	457786.587180	42.541696
3503.969964	457734.355262	42.546701
3503.960003	457694.279963	42.551706
3503.765171	457655.802003	42.556711
3504.230568	457608.922467	42.561716
3504.209738	457570.518445	42.566720
3504.130421	457519.978866	42.571725
3503.601102	457480.489916	42.576730
3503.961185	457436.611853	42.581735
3504.046594	457391.612558	42.586740
3503.867195	457351.056807	42.591744
3503.932678	457300.544660	42.596749
3503.709583	457256.655687	42.601754
3504.154874	457215.091552	42.606759
3504.143474	457167.424768	42.611764
3503.836806	457127.546145	42.616768
3503.739946	457078.070686	42.621773
3503.929167	457039.177372	42.626778
3503.777554	457001.500899	42.631783
3504.148120	456955.848858	42.636788
3503.719073	456907.740313	42.641792
3503.903430	456859.384369	42.646797
3503.733304	456827.327480	42.651802
3503.433676	456781.222623	42.656807
3503.769240	456742.761316	42.661812
3503.544701	456708.739095	42.666816
3503.689413	456660.287559	42.671821
3503.675543	456626.282998	42.676826
3503.714651	456579.669452	42.681831
3503.618817	456544.715990	42.686836
3503.332951	456503.365149	42.691840
3503.518377	456453.742781	42.696845
3503.415650	456423.850699	42.701850
3503.153585	456388.113101	42.706855
3503.659859	456344.968630	42.711860
3503.571659	456319.173180	42.716864
3503.380844	456282.260342	42.721869
3503.577620	456244.831658	42.726874
3503.597360	456209.910147	42.731879
3503.283143	456161.579250	42.736884
3503.428516	456137.973864	42.741888
3503.901079	456099.439218	42.746893
3503.491782	456060.687469	42.751898
3503.540935	456015.791483	42.756903
3503.362655	455984.341596	42.761908
3503.856911	455939.932827	42.766912
3503.865708	455903.342376	42.771917
3503.645137	455860.512248	42.776922
3503.792247	455828.201730	42.781927
3503.750282	455779.726198	42.786932
3503.601622	455745.740901	42.791937
3503.960838	455687.890893	42.796941
3503.563532	455653.944110	42.801946
3503.812597	455619.238775	42.806951
3504.139182	455573.438149	42.811956
3503.907193	455534.252778	42.816961
3503.595813	455491.587703	42.821965
3503.697172	455452.198451	42.826970
3503.606884	455417.494916	42.831975
3503.534584	455375.602091	42.836980
3503.376548	455343.793644	42.841985
3503.671927	455297.592285	42.846989
3503.615753	455260.959996	42.851994
3503.625614	455222.242383	42.856999
3503.806565	455189.419333	42.862004
3503.613771	455140.763070	42.867009
3503.806327	455097.816181	42.872013
3503.750646	455061.942541	42.877018
3503.902710	455018.849932	42.882023
3503.743484	454974.591024	42.887028
3503.382802	454945.040219	42.892033
3503.634566	454896.212880	42.897037
3503.424896	454856.010322	42.902042
3503.431994	454818.456282	42.907047
3503.312525	454779.302327	42.912052
3503.298781	454755.517403	42.917057
3503.476666	454706.144319	42.922061
3503.631727	454680.612267	42.927066
3503.461605	454645.059250	42.932071
3503.383972	454599.875708	42.937076
3503.250175	454570.187745	42.942081
3503.259068	454536.023756	42.947085
3503.454406	454509.321135	42.952090
3503.236964	454458.490541	42.957095
3503.535049	454428.684522	42.962100
3503.443967	454390.335066	42.967105
3503.264441	454349.165042	42.972109
3503.203137	454323.666143	42.977114
3503.304222	454292.675870	42.982119
3503.664697	454253.243614	42.987124
3503.697739	454219.631985	42.992129
3503.538132	454168.285435	42.997133
3503.631870	454139.776030	43.002138
3503.194779	454099.910808	43.007143
3503.649266	454066.992491	43.012148
3503.426981	454035.444739	43.017153
3503.712233	453986.812122	43.022157
3503.239205	453956.011823	43.027162
3503.196131	453921.095540	43.032167
3503.554968	453882.320678	43.037172
3503.430281	453852.731314	43.042177
3503.457528	453815.880587	43.047181
3503.505894	453786.517250	43.052186
3503.568408	453743.688527	43.057191
3503.470683	453702.048745	43.062196
3503.154067	453673.349376	43.067201
3503.427654	453629.728329	43.072205
3503.272707	453595.233721	43.077210
3503.221055	453559.153942	43.082215
3503.655411	453528.110468	43.087220
3503.361776	453497.939435	43.092225
3503.407120	453454.555930	43.097229
3503.292402	453415.499439	43.102234
3503.446524	453380.500788	43.107239
3503.728755	453347.506711	43.112244
3503.509019	453316.969569	43.117249
3503.595706	453263.304410	43.122253
3503.463794	453235.081735	43.127258
3503.485095	453191.802558	43.132263
3503.704499	453157.096997	43.137268
3503.435738	453120.797036	43.142273
3503.638659	453073.693177	43.147277
3503.766526	453041.481780	43.152282
3503.732404	453009.599225	43.157287
3503.546580	452962.707411	43.162292
3503.667528	452935.609068	43.167297
3503.540368	452882.178497	43.172301
3503.193239	452849.078967	43.177306
3503.440391	452812.090701	43.182311
3503.766417	452774.381459	43.187316
3503.342362	452741.597395	43.192321
3503.258956	452703.597402	43.197325
3503.407766	452675.735083	43.202330
3503.439835	452630.984989	43.207335
3503.663470	452592.177731	43.212340
3503.727100	452558.456958	43.217345
3503.719652	452509.865839	43.222349
3503.503151	452471.987296	43.227354
3503.329299	452430.811928	43.232359
3503.489021	452400.315392	43.237364
3503.253227	452359.149496	43.242369
3503.435025	452329.864219	43.247373
3503.255837	452303.722730	43.252378
3503.273724	452263.782573	43.257383
3503.303383	452222.979994	43.262388
3503.179340	452200.828567	43.267393
3503.318346	452157.680408	43.272397
3503.361221	452124.468220	43.277402
3503.361817	452085.087150	43.282407
3503.544957	452053.118454	43.287412
3503.439883	452024.434115	43.292417
3503.527217	451986.051693	43.297421
3503.441330	451956.503748	43.302426
3503.470065	451919.294524	43.307431
3503.569458	451873.367824	43.312436
3503.128062	451844.735531	43.317441
3503.272970	451805.483243	43.322445
3503.404768	451777.622167	43.327450
3503.166862	451738.935493	43.332455
3503.746925	451698.248540	43.337460
3503.486049	451677.585709	43.342465
3503.417458	451625.660827	43.347469
3503.581850	451587.569273	43.352474
3503.202263	451546.980690	43.357479
3503.520739	451512.155269	43.362484
3503.077109	451475.777922	43.367489
3502.573883	451440.827130	43.372493
3503.009835	451414.436753	43.377498
3503.291031	451391.360720	43.382503
3503.187736	451359.992176	43.387508
3502.856037	451335.290362	43.392513
3503.226567	451302.784960	43.397517
3503.449863	451274.250798	43.402522
3503.234964	451234.040839	43.407527
3503.557832	451203.516872	43.412532
3502.827976	451168.195848	43.417537
3503.248469	451121.255456	43.422541
3503.411078	451096.324528	43.427546
3502.953802	451056.708716	43.432551
3503.080276	451030.770901	43.437556
3503.170737	451010.558836	43.442561
3503.528983	450967.728036	43.447565
3503.071463	450933.832184	43.452570
3503.215218	450902.120665	43.457575
3503.531900	450863.902630	43.462580
3503.237668	450835.802654	43.467585
3503.614281	450788.513868	43.472589
3503.379317	450759.645224	43.477594
3503.114847	450723.491574	43.482599
3503.417725	450692.817983	43.487604
3503.005542	450669.443944	43.492609
3503.030642	450633.396918	43.497613
3503.092336	450605.291816	43.502618
3502.782530	450573.447806	43.507623
3503.234616	450546.193064	43.512628
3502.594165	450515.260984	43.517633
3502.878006	450473.807390	43.522637
3503.474413	450455.389004	43.527642
3502.839834	450424.050871	43.532647
3503.440584	450380.370969	43.537652
3503.231891	450358.281053	43.542657
3503.203117	450320.064995	43.547661
3503.272042	450283.605462	43.552666
3503.148740	450249.504437	43.557671
3503.711763	450227.193024	43.562676
3503.271891	450188.534426	43.567681
3503.292489	450143.172408	43.572685
3503.716986	450118.756229	43.577690
3502.913540	450079.698360	43.582695
3503.220922	450043.504976	43.587700
3503.174267	450024.477485	43.592705
3503.007015	449991.040919	43.597709
3503.068889	449959.087357	43.602714
3502.649698	449931.410401	43.607719
3502.601937	449900.638151	43.612724
3502.507888	449877.821064	43.617729
3502.941172	449851.530058	43.622733
3502.753010	449825.892586	43.627738
3502.389706	449798.105479	43.632743
3502.794488	449776.476252	43.637748
3502.769957	449750.711961	43.642753
3502.876880	449721.130325	43.647757
3502.662473	449700.002357	43.652762
3502.771639	449660.700313	43.657767
3503.161181	449635.529546	43.662772
3502.699155	449617.629386	43.667777
3502.926712	449577.954363	43.672781
3503.212268	449558.368433	43.677786
3503.291125	449522.108313	43.682791
3503.366641	449492.531189	43.687796
3503.112170	449462.549737	43.692801
3503.036966	449429.958437	43.697805
3503.118205	449396.785852	43.702810
3502.995011	449363.341264	43.707815
3503.450237	449329.806605	43.712820
3503.023574	449304.863641	43.717825
3503.305866	449265.635048	43.722829
3503.044220	449236.919987	43.727834
3502.729654	449206.744957	43.732839
3502.722799	449180.521465	43.737844
3502.774863	449158.592003	43.742849
3502.926203	449129.154363	43.747853
3502.873422	449099.697812	43.752858
3502.702298	449074.005993	43.757863
3503.054223	449041.195645	43.762868
3502.949096	449023.087475	43.767873
3503.045554	448986.519781	43.772877
3503.199413	448953.790723	43.777882
3503.009103	448925.469081	43.782887
3503.163089	448903.827211	43.787892
3502.741569	448872.959487	43.792897
3503.447618	448839.384889	43.797901
3503.148150	448795.588103	43.802906
3503.008270	448768.473422	43.807911
3503.138262	448727.647285	43.812916
3503.038260	448701.032573	43.817921
3503.151855	448667.701732	43.822925
3503.054760	448645.744231	43.827930
3502.855045	448615.297202	43.832935
3503.052720	448584.788282	43.837940
3503.193020	448561.730552	43.842945
3502.871407	448529.074715	43.847949
3502.577192	448499.199104	43.852954
3502.856435	448487.004704	43.857959
3503.087149	448443.630845	43.862964
3502.722482	448415.082393	43.867969
3502.799473	448394.768234	43.872973
3503.028222	448360.558226	43.877978
3502.799379	448325.558673	43.882983
3502.921570	448307.313156	43.887988
3502.707157	448277.475390	43.892993
3502.972741	448248.980488	43.897997
3503.078952	448216.460028	43.903002
3502.691022	448196.926800	43.908007
3502.803639	448170.784512	43.913012
3502.523777	448138.374618	43.918017
3502.834805	448106.227122	43.923021
3502.953611	448092.133513	43.928026
3502.773519	448064.315225	43.933031
3503.310009	448038.359934	43.938036
3502.742952	448011.563741	43.943041
3502.783071	447972.521922	43.948045
3502.801276	447948.520449	43.953050
3502.876981	447931.648790	43.958055
3502.640997	447903.079507	43.963060
3502.422377	447892.126667	43.968065
3502.940547	447851.339413	43.973069
3502.634489	447826.831309	43.978074
3502.467643	447796.074008	43.983079
3502.993704	447764.803788	43.988084
3502.686838	447749.763549	43.993089
3502.983526	447721.870544	43.998093
3503.018256	447697.967430	44.003098
3502.886972	447666.748703	44.008103
3502.957026	447637.625074	44.013108
3502.840304	447612.175868	44.018113
3502.469263	447578.057721	44.023117
3502.628320	447554.995794	44.028122
3502.494710	447532.789474	44.033127
3502.990654	447510.282637	44.038132
3502.907323	447486.093830	44.043137
3503.019375	447455.849494	44.048141
3502.857143	447428.078084	44.053146
3502.707736	447414.785154	44.058151
3502.783741	447381.609696	44.063156
3502.500998	447359.325108	44.068161
3502.822233	447322.465926	44.073165
3503.134349	447299.481121	44.078170
3502.663741	447271.706828	44.083175
3502.818358	447240.949195	44.088180
3502.912566	447228.073904	44.093185
3502.770170	447181.565299	44.098189
3502.777660	447158.931511	44.103194
3502.697227	447142.032785	44.108199
3502.505818	447117.657780	44.113204
3502.275432	447097.086211	44.118209
3502.593497	447073.543243	44.123213
3502.591072	447053.290576	44.128218
3502.711028	447030.791025	44.133223
3502.864128	446999.577531	44.138228
3502.817475	446969.205187	44.143233
3502.683634	446943.099488	44.148237
3502.914438	446920.481287	44.153242
3502.900308	446895.723970	44.158247
3502.858526	446860.844385	44.163252
3502.931309	446836.731689	44.168257
3503.083124	446808.961098	44.173261
3503.244439	446774.404173	44.178266
3502.575722	446747.672567	44.183271
3502.755317	446707.087340	44.188276
3502.466948	446695.182604	44.193281
3502.619164	446662.247144	44.198285
3502.599945	446647.667564	44.203290
3502.524751	446623.780146	44.208295
3502.666654	446594.896838	44.213300
3502.840141	446576.996041	44.218305
3503.008996	446545.678053	44.223309
3502.959105	446518.292844	44.228314
3502.526830	446497.600114	44.233319
3502.913741	446474.197563	44.238324
3502.860592	446450.711559	44.243329
3502.609504	446427.053791	44.248333
3502.583316	446406.348399	44.253338
3502.483884	446372.489532	44.258343
3502.422768	446350.979368	44.263348
3502.317026	446328.868513	44.268353
3502.602895	446313.886752	44.273357
3502.585332	446289.888662	44.278362
3502.588275	446270.241903	44.283367
3502.662771	446245.318011	44.288372
3502.926550	446223.048257	44.293377
3502.561687	446191.407641	44.298381
3502.895473	446170.443428	44.303386
3502.858554	446145.030391	44.308391
3502.904822	446112.009158	44.313396
3502.580568	446094.235978	44.318401
3502.621014	446061.519370	44.323405
3502.925043	446030.280736	44.328410
3502.578598	446005.422022	44.333415
3502.884010	445977.524998	44.338420
3502.837967	445953.784075	44.343425
3502.585583	445920.505160	44.348429
3502.630215	445907.332842	44.353434
3502.746445	445868.730397	44.358439
3503.252173	445839.738647	44.363444
3502.439568	445829.484624	44.368449
3502.472575	445804.667860	44.373453
3502.749216	445775.863566	44.378458
3502.605331	445759.378520	44.383463
3502.953249	445725.853931	44.388468
3502.734549	445702.848452	44.393473
3502.601989	445672.436687	44.398477
3502.577109	445663.072710	44.403482
3502.639687	445632.326697	44.408487
3502.930193	445612.431940	44.413492
3502.976248	445578.093240	44.418497
3502.831287	445554.164647	44.423501
3503.092692	445526.172514	44.428506
3502.562712	445498.506032	44.433511
3502.735471	445463.742310	44.438516
3502.493301	445445.803817	44.443521
3502.508319	445424.685811	44.448525
3502.760230	445396.492411	44.453530
3502.494511	445368.075696	44.458535
3502.807220	445337.796635	44.463540
3502.756354	445314.106271	44.468545
3502.966228	445288.856192	44.473549
3502.955585	445259.741335	44.478554
3502.709728	445235.220382	44.483559
3502.664781	445198.819009	44.488564
3502.550987	445184.961905	44.493569
3502.775293	445161.380437	44.498573
3503.153319	445133.065733	44.503578
3503.096363	445111.958569	44.508583
3503.034801	445077.382492	44.513588
3502.932164	445055.168343	44.518593
3502.795089	445028.554041	44.523597
3502.876768	445003.222243	44.528602
3502.607053	444967.969422	44.533607
3503.096213	444936.345658	44.538612
3502.668370	444918.131714	44.543617
3502.973525	444878.535667	44.548621
3502.468779	444856.231936	44.553626
3502.291701	444837.219316	44.558631
3502.415147	444814.716504	44.563636
3502.556753	444787.298911	44.568641
3502.907763	444771.141075	44.573645
3502.826698	444747.657236	44.578650
3502.826218	444722.641669	44.583655
3502.914708	444695.029651	44.588660
3502.647823	444672.435489	44.593665
3502.649865	444648.482842	44.598669
3502.921399	444611.575311	44.603674
3502.462563	444589.922419	44.608679
3503.057631	444560.205810	44.613684
3503.009291	444541.932438	44.618689
3502.799216	444507.783516	44.623693
3502.886586	444481.538610	44.628698
3502.680526	444456.807870	44.633703
3502.566402	444435.759466	44.638708
3502.584067	444418.944243	44.643713
3502.635432	444395.793824	44.648717
3502.902486	444364.355561	44.653722
3502.452574	444337.940862	44.658727
3502.896057	444317.413228	44.663732
3502.279669	444295.075550	44.668737
3502.449451	444268.007280	44.673741
3502.702674	444252.016127	44.678746
3502.361511	444226.192023	44.683751
3502.741855	444199.344087	44.688756
3502.286443	444183.058026	44.693761
3502.193670	444150.713232	44.698765
3502.329268	444126.587205	44.703770
3502.440516	444118.011503	44.708775
3502.525595	444086.753007	44.713780
3502.225717	444083.912983	44.718785
3502.711011	444046.059533	44.723789
3502.926218	444035.441997	44.728794
3502.717664	444006.102755	44.733799
3502.561633	443984.250109	44.738804
3502.403894	443956.219537	44.743809
3502.365852	443939.159343	44.748813
3502.532701	443910.976911	44.753818
3502.383818	443902.745433	44.758823
3502.464540	443864.498801	44.763828
3502.638867	443857.128545	44.768833
3502.821324	443822.157658	44.773837
3502.607139	443790.995872	44.778842
3502.652927	443770.276314	44.783847
3502.703427	443736.642471	44.788852
3502.592819	443715.542058	44.793857
3502.582505	443697.110009	44.798861
3502.892061	443682.730124	44.803866
3502.592711	443647.428750	44.808871
3502.209651	443626.016141	44.813876
3502.297073	443607.518152	44.818881
3502.381683	443586.792347	44.823885
3502.647505	443563.050456	44.828890
3502.507303	443552.285382	44.833895
3502.837025	443522.000700	44.838900
3502.627255	443506.435445	44.843905
3502.570971	443474.387642	44.848909
3502.758015	443453.797675	44.853914
3502.160833	443433.177793	44.858919
3502.872706	443407.998955	44.863924
3502.684720	443384.631307	44.868929
3502.922276	443362.463468	44.873933
3502.742854	443334.182117	44.878938
3502.776239	443304.247047	44.883943
3503.133309	443273.349994	44.888948
3502.465438	443241.447602	44.893953
3502.629326	443227.039391	44.898957
3503.155899	443195.609405	44.903962
3502.649703	443170.974292	44.908967
3502.923048	443147.889057	44.913972
3502.808528	443125.016078	44.918977
3502.488712	443094.882419	44.923981
3502.650519	443064.572478	44.928986
3502.393979	443042.227929	44.933991
3502.784582	443026.264986	44.938996
3502.604290	443002.338582	44.944001
3502.397481	442984.341549	44.949005
3502.743298	442962.865394	44.954010
3502.595230	442938.174242	44.959015
3502.776778	442901.530527	44.964020
3502.752774	442888.670599	44.969025
3502.745128	442862.286256	44.974029
3502.910430	442832.836337	44.979034
3502.478743	442810.974558	44.984039
3502.684137	442775.491692	44.989044
3502.241549	442765.836739	44.994049
3502.199727	442739.761404	44.999053
3502.480372	442726.499448	45.004058
3502.545659	442693.823652	45.009063
3502.463686	442660.816205	45.014068
3502.478868	442652.457352	45.019073
3502.470637	442638.581912	45.024077
3502.419356	442606.126678	45.029082
3502.461036	442592.749880	45.034087
3502.350119	442563.545096	45.039092
3502.593658	442545.984003	45.044097
3502.358203	442522.470723	45.049101
3502.454388	442502.147064	45.054106
3502.646565	442481.757802	45.059111
3502.697840	442452.679539	45.064116
3502.652569	442440.480993	45.069121
3502.701678	442417.480391	45.074125
3502.702663	442380.813105	45.079130
3502.890892	442372.680424	45.084135
3502.628737	442335.395611	45.089140
3502.799227	442310.400829	45.094145
3502.349012	442288.085511	45.099149
3502.802984	442255.297817	45.104154
3502.558288	442238.926608	45.109159
3502.564511	442214.463713	45.114164
3502.534217	442201.097835	45.119169
3502.648295	442178.137474	45.124173
3503.065681	442149.609513	45.129178
3502.677388	442136.046069	45.134183
3502.707528	442100.386608	45.139188
3502.686614	442073.496755	45.144193
3502.481820	442049.724877	45.149197
3503.012858	442022.445184	45.154202
3502.572004	442003.217472	45.159207
3502.861552	441970.404219	45.164212
3502.449448	441945.145084	45.169217
3502.512245	441920.065246	45.174221
3502.595446	441891.690188	45.179226
3502.474666	441880.465306	45.184231
3502.611779	441852.436324	45.189236
3502.821576	441830.828095	45.194241
3502.544394	441802.660921	45.199245
3502.539400	441781.440585	45.204250
3502.527621	441762.449735	45.209255
3502.887478	441733.828800	45.214260
3502.492445	441713.682017	45.219265
3502.625981	441684.083288	45.224269
3502.921815	441666.614525	45.229274
3502.559294	441639.017501	45.234279
3502.546789	441611.011439	45.239284
3502.524032	441596.529719	45.244289
3502.726170	441569.300548	45.249293
3502.798058	441545.231737	45.254298
3502.529446	441513.011011	45.259303
3502.475741	441501.978053	45.264308
3502.334158	441472.168564	45.269313
3502.277923	441454.855686	45.274317
3502.503550	441440.841669	45.279322
3502.345419	441415.339705	45.284327
3502.525796	441391.507052	45.289332
3502.489381	441372.063810	45.294337
3502.497335	441349.372185	45.299341
3502.825397	441324.148974	45.304346
3502.127484	441307.847474	45.309351
3502.394966	441279.037628	45.314356
3502.607794	441269.685089	45.319361
3502.363773	441238.878209	45.324365
3502.359106	441220.493479	45.329370
3502.201328	441197.776812	45.334375
3502.317968	441181.905577	45.339380
3502.200166	441155.130777	45.344385
3502.140326	441139.793453	45.349389
3502.557317	441129.497404	45.354394
3502.203089	441098.403551	45.359399
3502.095911	441075.678862	45.364404
3502.300059	441057.514721	45.369409
3502.081055	441042.100787	45.374413
3502.550216	441012.955257	45.379418
3502.453490	441003.346864	45.384423
3502.447545	440985.772483	45.389428
3502.679422	440958.385851	45.394433
3502.719774	440938.069183	45.399437
3502.719601	440912.440656	45.404442
3502.455716	440900.427072	45.409447
3502.910469	440888.757491	45.414452
3502.620090	440859.071479	45.419457
3502.522156	440833.559356	45.424461
3502.615702	440801.939490	45.429466
3502.566312	440795.362581	45.434471
3502.492195	440758.855750	45.439476
3502.454782	440739.665255	45.444481
3502.869218	440707.438152	45.449485
3502.847702	440682.623026	45.454490
3502.539191	440670.008442	45.459495
3502.589567	440636.622278	45.464500
3502.193045	440615.968046	45.469505
3502.440783	440596.986281	45.474509
3502.541233	440573.367627	45.479514
3502.322373	440560.283170	45.484519
3502.541675	440524.895174	45.489524
3502.796404	440507.634331	45.494529
3502.427830	440479.935240	45.499533
3502.811787	440456.322972	45.504538
3502.668041	440429.095322	45.509543
3502.764281	440405.173210	45.514548
3502.593350	440379.975733	45.519553
3502.202141	440363.524380	45.524557
3502.700396	440341.616298	45.529562
3502.422001	440315.878301	45.534567
3502.662016	440301.000137	45.539572
3502.570820	440262.013119	45.544577
3502.644828	440244.172349	45.549581
3502.982461	440226.847698	45.554586
3502.538159	440205.795243	45.559591
3502.580270	440175.853808	45.564596
3502.634004	440157.560252	45.569601
3502.545198	440126.879346	45.574605
3502.628079	440104.377162	45.579610
3502.797185	440087.382515	45.584615
3502.758945	440067.229089	45.589620
3502.770676	440041.344267	45.594625
3502.753883	440016.679482	45.599629
3502.823571	439985.669774	45.604634
3502.751571	439958.886143	45.609639
3502.756411	439926.721443	45.614644
3502.633978	439905.719869	45.619649
3502.475041	439886.192852	45.624653
3502.545635	439868.200302	45.629658
3502.275045	439846.917807	45.634663
3502.378731	439823.804228	45.639668
3502.483980	439792.332802	45.644673
3502.421396	439785.099116	45.649677
3502.669973	439760.949874	45.654682
3502.087973	439737.892239	45.659687
3502.329919	439720.024840	45.664692
3502.545282	439694.259811	45.669697
3502.506015	439677.905048	45.674701
3502.607397	439651.549870	45.679706
3502.455561	439630.907132	45.684711
3502.620243	439604.440733	45.689716
3502.754149	439572.356651	45.694721
3502.808868	439547.730777	45.699725
3502.676886	439522.272828	45.704730
3502.240977	439513.222982	45.709735
3502.505902	439489.526723	45.714740
3502.294686	439468.133255	45.719745
3502.741136	439442.534535	45.724749
3502.444962	439428.802833	45.729754
3502.343343	439404.555672	45.734759
3502.337782	439382.724880	45.739764
3502.595921	439361.258253	45.744769
3502.391696	439349.437004	45.749773
3502.459482	439325.720565	45.754778
3502.550707	439303.975928	45.759783
3502.442464	439271.169217	45.764788
3502.399535	439256.030339	45.769793
3502.050271	439249.904781	45.774797
3501.625295	439217.248571	45.779802
3501.993173	439203.109449	45.784807
3502.236935	439168.525562	45.789812
3501.954065	439097.654131	45.794817
3501.918025	438993.717560	45.799821
3501.490303	438834.830603	45.804826
3501.462578	438624.414539	45.809831
3501.203377	438369.252490	45.814836
3500.776550	438078.602874	45.819841
3500.180226	437740.509201	45.824845
3499.987452	437352.498829	45.829850
3498.999296	436921.391715	45.834855
3498.497481	436434.421594	45.839860
3497.471617	435929.586222	45.844865
3496.767048	435370.984105	45.849869
3495.625997	434764.200388	45.854874
3494.504255	434120.559734	45.859879
3493.423872	433449.175484	45.864884
3492.365100	432731.097107	45.869889
3491.023783	431971.890183	45.874893
3489.932445	431171.568513	45.879898
3488.668348	430340.835121	45.884903
3487.425616	429458.674983	45.889908
3485.725239	428541.069906	45.894913
3484.340439	427588.097586	45.899917
3482.912276	426603.255718	45.904922
3481.159893	425581.311922	45.909927
3479.118716	424519.467284	45.914932
3477.534348	423433.720580	45.919937
3475.522499	422307.222458	45.924941
3473.873958	421146.687983	45.929946
3471.471849	419969.625960	45.934951
3469.700426	418746.206476	45.939956
3467.813149	417512.084841	45.944961
3465.100978	416235.827327	45.949965
3463.295964	414936.733216	45.954970
3460.749734	413617.439167	45.959975
3458.761853	412250.756183	45.964980
3456.495006	410884.791473	45.969985
3453.995608	409479.058056	45.974989
3451.776462	408049.246487	45.979994
3448.942132	406592.346677	45.984999
3446.502822	405120.779775	45.990004
3443.922515	403623.464165	45.995009
3441.449878	402115.833865	46.000013
3438.632582	400575.578457	46.005018
3435.521141	399034.251524	46.010023
3433.171317	397456.567556	46.015028
3430.673504	395870.629283	46.020033
3427.655987	394261.265584	46.025037
3425.020812	392636.353193	46.030042
3422.270644	390977.335649	46.035047
3419.327903	389320.799989	46.040052
3416.523392	387639.912715	46.045057
3413.542914	385951.856627	46.050061
3410.662756	384233.305162	46.055066
3407.533539	382517.775096	46.060071
3404.604423	380770.103679	46.065076
3401.260424	379016.234489	46.070081
3397.798685	377260.870731	46.075085
3395.039951	375491.059155	46.080090
3391.414718	373709.912860	46.085095
3388.396677	371914.991676	46.090100
3384.842000	370114.246049	46.095105
3381.680654	368305.473718	46.100109
3378.776083	366488.899150	46.105114
3375.431885	364660.819395	46.110119
3371.987534	362824.001542	46.115124
3368.334847	360975.158764	46.120129
3365.323440	359129.635112	46.125133
3362.022275	357263.204492	46.130138
3358.232063	355400.549948	46.135143
3354.939465	353529.522817	46.140148
3351.327269	351649.386157	46.145153
3347.673314	349774.510588	46.150157
3344.531775	347886.864052	46.155162
3340.702133	346003.768678	46.160167
3337.428015	344095.743225	46.165172
3334.142154	342195.674189	46.170177
3330.382152	340288.023606	46.175181
3326.871836	338369.220896	46.180186
3323.099645	336464.547681	46.185191
3319.493181	334548.432823	46.190196
3316.039660	332624.642450	46.195201
3312.142342	330711.990024	46.200205
3308.826790	328785.366596	46.205210
3304.821180	326869.236948	46.210215
3301.297804	324948.209699	46.215220
3297.752774	323029.716384	46.220225
3294.148418	321089.774305	46.225229
3290.189383	319155.371287	46.230234
3286.380050	317242.409591	46.235239
3282.897375	315307.992876	46.240244
3279.331110	313378.010885	46.245249
3275.336462	311449.440608	46.250253
3271.664234	309511.352063	46.255258
3267.785865	307597.190804	46.260263
3264.176271	305664.030985	46.265268
3260.601591	303723.081226	46.270273
3256.054318	301799.695813	46.275277
3252.684472	299878.069016	46.280282
3249.065439	297964.558925	46.285287
3245.162945	296033.668813	46.290292
3241.635149	294115.765366	46.295297
3237.792605	292189.067281	46.300301
3233.825979	290255.531383	46.305306
3230.197860	288345.482362	46.310311
3226.458020	286426.510162	46.315316
3222.344995	284520.754270	46.320321
3218.816253	282615.466274	46.325325
3214.805074	280711.119429	46.330330
3210.649495	278805.778830	46.335335
3207.129642	276911.164037	46.340340
3203.248373	275012.384906	46.345345
3199.551207	273116.589169	46.350349
3195.589446	271221.582345	46.355354
3191.373714	269341.853044	46.360359
3187.864046	267454.820940	46.365364
3184.238184	265570.469839	46.370369
3179.986460	263689.364668	46.375373
3176.197398	261813.120388	46.380378
3172.130042	259949.468341	46.385383
3168.490019	258088.140041	46.390388
3164.618997	256236.242824	46.395393
3160.392233	254384.706508	46.400397
3156.709772	252534.844208	46.405402
3152.915659	250693.432008	46.410407
3149.171830	248845.675427	46.415412
3145.464881	247016.638079	46.420417
3140.834501	245194.272332	46.425421
3137.145117	243356.641817	46.430426
3133.020927	241535.695276	46.435431
3129.024763	239722.687691	46.440436
3125.521732	237919.474007	46.445441
3121.109479	236123.421558	46.450445
3117.717894	234319.663363	46.455450
3113.160376	232533.449648	46.460455
3109.249323	230755.840485	46.465460
3105.420749	228983.206599	46.470465
3101.236022	227220.685980	46.475469
3097.595881	225465.873081	46.480474
3093.452725	223706.808981	46.485479
3089.804841	221972.221543	46.490484
3085.538345	220228.768118	46.495489
3081.954120	218502.149494	46.500493
3077.979365	216774.399939	46.505498
3073.995002	215053.891592	46.510503
3070.091665	213342.980083	46.515508
3066.144917	211645.124101	46.520513
3062.159986	209940.305741	46.525517
3058.025609	208243.951865	46.530522
3054.238164	206565.740460	46.535527
3050.418421	204887.929356	46.540532
3046.221001	203218.239158	46.545537
3041.947516	201566.912617	46.550541
3038.380837	199904.770663	46.555546
3034.085268	198265.857946	46.560551
3030.057719	196630.563322	46.565556
3026.206861	195008.375344	46.570561
3021.734424	193389.792739	46.575565
3017.759559	191784.624720	46.580570
3013.865922	190198.156909	46.585575
3009.597349	188617.091513	46.590580
3005.584701	187038.530018	46.595585
3001.448748	185475.391612	46.600589
2997.550296	183915.907126	46.605594
2993.278076	182372.598477	46.610599
2989.133267	180842.612354	46.615604
2984.997345	179314.203816	46.620609
2980.667077	177818.086863	46.625613
2976.671300	176327.303790	46.630618
2972.265647	174838.024505	46.635623
2968.311276	173379.662645	46.640628
2964.142409	171919.973892	46.645633
2959.638757	170489.096434	46.650637
2955.259219	169055.490552	46.655642
2951.244789	167645.036406	46.660647
2946.717242	166245.268251	46.665652
2942.442648	164872.054215	46.670657
2937.818374	163500.997484	46.675661
2933.345030	162155.300574	46.680666
2929.233845	160835.095097	46.685671
2924.807892	159535.076096	46.690676
2919.750674	158247.439282	46.695681
2915.193351	156983.717356	46.700685
2910.525340	155728.592054	46.705690
2905.898205	154518.908728	46.710695
2901.244962	153325.175695	46.715700
2896.180445	152160.458364	46.720705
2891.007832	151020.954016	46.725709
2885.928786	149901.527119	46.730714
2880.957058	148824.214851	46.735719
2876.028162	147775.396477	46.740724
2871.322991	146720.138317	46.745729
2866.136677	145665.981867	46.750733
2861.579624	144699.228719	46.755738
2856.683319	143766.227502	46.760743
2852.143172	142850.454589	46.765748
2847.538665	141941.070546	46.770753
2843.214189	141079.423368	46.775757
2838.608082	140213.674990	46.780762
2834.240044	139386.557451	46.785767
2830.222600	138572.885897	46.790772
2826.377820	137768.667150	46.795777
2821.961944	136989.143334	46.800781
2817.854118	136211.645795	46.805786
2813.458431	135472.104625	46.810791
2809.786328	134733.429821	46.815796
2806.117206	134008.060612	46.820801
2802.409235	133298.839780	46.825805
2798.640145	132586.001677	46.830810
2795.140381	131890.815182	46.835815
2791.242960	131189.023404	46.840820
2787.723572	130509.037847	46.845825
2783.800685	129834.163089	46.850829
2780.369607	129162.924044	46.855834
2776.499271	128498.823521	46.860839
2773.214105	127827.112485	46.865844
2769.349107	127167.407865	46.870849
2765.184657	126514.209005	46.875853
2762.228677	125851.802026	46.880858
2758.600796	125210.076607	46.885863
2755.286440	124560.032791	46.890868
2751.583847	123922.918153	46.895873
2747.867440	123283.170447	46.900877
2744.599575	122642.180478	46.905882
2741.155708	122017.977572	46.910887
2737.813193	121383.187835	46.915892
2734.078218	120751.597972	46.920897
2730.591246	120129.733844	46.925901
2726.827491	119488.237043	46.930906
2723.318588	118857.520528	46.935911
2719.734023	118247.096334	46.940916
2716.051060	117626.002901	46.945921
2712.034965	117005.086009	46.950925
2708.737938	116398.512754	46.955930
2704.370890	115792.764408	46.960935
2700.578264	115189.225377	46.965940
2697.036515	114608.697246	46.970945
2692.977763	114027.877332	46.975949
2689.430383	113448.474746	46.980954
2685.592266	112863.570378	46.985959
2681.452898	112295.963173	46.990964
2678.207683	111742.313199	46.995969
2673.962716	111190.823508	47.000973
2670.317176	110623.483933	47.005978
2666.177336	110083.539315	47.010983
2662.276970	109558.949016	47.015988
2658.660795	109014.960052	47.020993
2654.743623	108496.503424	47.025997
2651.215703	107969.069534	47.031002
2647.780245	107457.431191	47.036007
2643.860215	106953.821194	47.041012
2640.181015	106436.731504	47.046017
2636.644782	105951.649267	47.051021
2633.478517	105430.071249	47.056026
2629.852620	104937.021703	47.061031
2626.249323	104439.717495	47.066036
2623.041481	103933.054408	47.071041
2619.465229	103438.354013	47.076045
2615.993381	102932.065029	47.081050
2612.688015	102433.269966	47.086055
2608.741898	101942.475456	47.091060
2605.673377	101445.132959	47.096065
2601.737242	100945.950255	47.101069
2598.618429	100452.189588	47.106074
2595.187736	99961.586177	47.111079
2592.143256	99468.693220	47.116084
2588.647087	98953.890778	47.121089
2584.975865	98466.397874	47.126093
2581.515876	97949.813970	47.131098
2578.059305	97453.432268	47.136103
2574.688121	96947.856720	47.141108
2571.279582	96445.065530	47.146113
2567.883514	95953.044321	47.151117
2564.176277	95433.363071	47.156122
2560.993593	94935.796700	47.161127
2557.428411	94427.381992	47.166132
2553.861090	93910.360363	47.171137
2550.447079	93414.061686	47.176141
2547.609492	92897.667839	47.181146
2543.875330	92385.335926	47.186151
2540.321148	91874.229872	47.191156
2537.019967	91359.751295	47.196161
2533.315548	90843.895737	47.201165
2529.910337	90313.822681	47.206170
2526.481113	89809.771253	47.211175
2523.149095	89283.694645	47.216180
2519.601782	88772.653024	47.221185
2516.254874	88260.115248	47.226189
2512.736321	87723.054724	47.231194
2509.426750	87208.979444	47.236199
2505.768555	86680.293931	47.241204
2502.358903	86149.699112	47.246209
2498.640839	85641.241311	47.251213
2495.534886	85112.193486	47.256218
2492.167553	84588.874465	47.261223
2488.699907	84056.764574	47.266228
2484.888066	83514.720922	47.271233
2481.330305	82985.681004	47.276237
2478.072959	82453.733428	47.281242
2474.758966	81935.421455	47.286247
2470.875312	81397.024188	47.291252
2467.931792	80859.405458	47.296257
2464.644282	80321.456837	47.301261
2461.074069	79775.154355	47.306266
2457.442571	79232.707857	47.311271
2453.809097	78701.728384	47.316276
2450.576996	78154.528919	47.321281
2446.684503	77617.031819	47.326285
2443.046992	77071.123589	47.331290
2439.770115	76534.047293	47.336295
2436.311604	75989.961654	47.341300
2433.173046	75441.049540	47.346305
2429.606641	74905.257043	47.351309
2426.350411	74350.785213	47.356314
2422.642623	73802.680880	47.361319
2419.085418	73247.593058	47.366324
2415.627904	72691.447387	47.371329
2412.239452	72158.196563	47.376333
2408.296076	71614.351642	47.381338
2404.728752	71055.768841	47.386343
2401.409220	70508.231070	47.391348
2398.224741	69962.162923	47.396353
2394.276889	69411.819402	47.401357
2390.909976	68850.148435	47.406362
2387.628455	68309.475257	47.411367
2383.906766	67757.766993	47.416372
2380.743839	67203.457284	47.421377
2377.045035	66651.350362	47.426381
2373.467485	66099.687206	47.431386
2369.884627	65546.640482	47.436391
2366.310582	64993.014206	47.441396
2363.119294	64443.573938	47.446401
2359.600180	63889.170042	47.451405
2356.163847	63324.978999	47.456410
2352.753158	62785.065813	47.461415
2348.873770	62221.114712	47.466420
2345.680042	61661.124993	47.471425
2342.390373	61110.187049	47.476429
2338.773765	60546.518898	47.481434
2335.603935	59986.772998	47.486439
2331.710344	59427.672903	47.491444
2328.206146	58872.383124	47.496449
2324.990698	58304.541717	47.501453
2321.513242	57742.839481	47.506458
2318.088508	57176.821146	47.511463
2314.239599	56617.087494	47.516468
2311.224962	56048.620908	47.521473
2307.236175	55485.464956	47.526477
2304.026067	54921.122608	47.531482
2300.357966	54350.996489	47.536487
2297.089258	53783.175666	47.541492
2293.692350	53217.031593	47.546497
2290.187765	52653.569675	47.551501
2286.449744	52078.218827	47.556506
2282.927674	51513.600888	47.561511
2279.018086	50940.182588	47.566516
2276.114999	50369.508030	47.571521
2272.606608	49803.064789	47.576525
2268.791353	49231.228352	47.581530
2265.534925	48656.452294	47.586535
2261.991542	48092.365555	47.591540
2258.881489	47520.614425	47.596545
2255.107619	46953.243023	47.601549
2251.664423	46370.746488	47.606554
2248.000373	45798.085015	47.611559
2244.566513	45225.351581	47.616564
2241.223604	44654.559179	47.621569
2237.368845	44087.646888	47.626573
2234.047513	43515.992481	47.631578
2230.849923	42929.641115	47.636583
2227.203425	42357.807222	47.641588
2223.763746	41775.836043	47.646593
2219.739664	41203.444155	47.651597
2216.450958	40617.872380	47.656602
2212.955747	40047.298897	47.661607
2209.308467	39473.410107	47.666612
2206.020407	38893.425921	47.671617
2202.752968	38323.439273	47.676621
2198.881947	37738.688845	47.681626
2195.299094	37169.498227	47.686631
2191.730566	36595.192014	47.691636
2188.169086	36018.624405	47.696641
2184.624435	35457.486131	47.701645
2181.047578	34876.432223	47.706650
2177.689761	34303.150336	47.711655
2174.317768	33739.286143	47.716660
2170.841114	33157.909026	47.721665
2167.068935	32590.791352	47.726669
2163.445514	32016.066747	47.731674
2159.651934	31447.012396	47.736679
2155.991485	30885.139725	47.741684
2152.476552	30312.593800	47.746689
2148.962709	29768.752216	47.751693
2145.377246	29198.086008	47.756698
2141.811785	28649.054001	47.761703
2137.932148	28089.313194	47.766708
2134.673811	27526.969100	47.771713
2130.645003	26982.229817	47.776717
2126.807114	26425.639425	47.781722
2123.634389	25889.065032	47.786727
2119.973102	25348.500643	47.791732
2116.635731	24794.614426	47.796737
2112.549801	24262.717513	47.801741
2108.648044	23726.371332	47.806746
2104.559868	23202.346155	47.811751
2100.267185	22692.639396	47.816756
2096.026776	22186.390089	47.821761
2092.151376	21700.634014	47.826765
2088.424899	21208.570171	47.831770
2084.382732	20735.418889	47.836775
2080.489591	20254.889086	47.841780
2076.812205	19795.854370	47.846785
2072.654633	19336.252760	47.851789
2068.935999	18884.694584	47.856794
2065.440036	18439.458539	47.861799
2061.496222	18003.485977	47.866804
2057.982899	17552.123155	47.871809
2053.925914	17142.816210	47.876813
2050.610400	16717.300674	47.881818
2046.992645	16283.019782	47.886823
2043.214021	15872.813060	47.891828
2040.173396	15452.377479	47.896833
2036.301153	15047.455944	47.901837
2032.895828	14620.832523	47.906842
2028.911035	14218.836824	47.911847
2025.240253	13807.046111	47.916852
2022.077970	13392.468767	47.921857
2018.751001	12995.322874	47.926861
2015.128044	12591.716046	47.931866
2011.352318	12193.001112	47.936871
2007.876890	11803.191054	47.941876
2004.412861	11398.499205	47.946881
2000.483617	11015.132769	47.951885
1997.131981	10623.510891	47.956890
1993.301273	10234.212920	47.961895
1989.662726	9861.464016	47.966900
1985.907561	9484.521329	47.971905
1982.216884	9111.162499	47.976909
1978.410837	8753.196221	47.981914
1974.640006	8394.614176	47.986919
1970.562955	8048.038114	47.991924
1966.974744	7705.291798	47.996929
1962.363181	7380.542583	48.001933
1958.341869	7048.912160	48.006938
1954.480145	6727.529699	48.011943
1950.618706	6424.334653	48.016948
1947.202576	6116.302866	48.021953
1942.542553	5834.034356	48.026957
1938.650034	5541.989060	48.031962
1935.002320	5275.743051	48.036967
1930.963601	5004.286459	48.041972
1927.487207	4733.550190	48.046977
1923.772772	4477.873587	48.051981
1920.244791	4214.966167	48.056986
1916.857060	3970.599842	48.061991
1913.248719	3731.970132	48.066996
1909.510066	3485.905598	48.072001
1905.540172	3239.627267	48.077005
1902.154232	2998.245055	48.082010
1898.713038	2768.436567	48.087015
1895.109124	2539.352449	48.092020
1891.718558	2300.663501	48.097025
1888.012522	2075.391779	48.102029
1884.702055	1853.215844	48.107034
1881.021060	1642.136278	48.112039
1877.371573	1424.837161	48.117044
1873.926997	1200.931049	48.122049
1870.233662	990.715352	48.127053
1866.439241	775.655070	48.132058
1862.895508	581.784214	48.137063
1858.787631	384.583255	48.142068
1854.774667	196.218637	48.147073
1848.871846	58.373749	48.152077
1837.839021	104.198979	48.157082
1830.162070	98.325899	48.162087
1824.969479	100.187385	48.167092
1822.395262	97.357702	48.172097
1819.596544	96.514964	48.177101
1817.924968	102.336725	48.182106
1815.446578	99.131465	48.187111
1812.623118	99.102486	48.192116
1809.758590	104.325318	48.197121
1806.024256	103.413066	48.202125
1802.919223	99.118949	48.207130
1799.679785	104.757629	48.212135
1795.683681	105.063017	48.217140
1792.833957	100.596289	48.222145
1789.810892	105.685611	48.227149
1786.353916	98.073765	48.232154
1783.057431	102.465335	48.237159
1779.424580	106.611869	48.242164
1776.149095	102.942222	48.247169
1772.147243	108.728039	48.252173
1768.754366	111.831168	48.257178
1765.675466	103.069003	48.262183
1762.247495	106.544583	48.267188
1759.372500	100.803656	48.272193
1756.300212	106.758003	48.277197
1752.462458	104.966525	48.282202
1748.883013	104.511055	48.287207
1745.043547	106.851638	48.292212
1742.080662	92.810190	48.297217
1738.024552	104.261147	48.302221
1734.696541	115.753810	48.307226
1731.655593	93.467251	48.312231
1728.237145	104.518411	48.317236
1724.739889	97.833481	48.322241
1721.269050	102.824819	48.327245
1717.646466	101.993258	48.332250
1714.302393	101.317664	48.337255
1710.667650	102.142611	48.342260
1707.864262	94.198104	48.347265
1704.270909	102.353228	48.352269
1700.209507	97.344283	48.357274
1696.900771	103.041207	48.362279
1693.255143	99.454490	48.367284
1690.292852	94.350409	48.372289
1686.890160	104.633501	48.377293
1683.236053	97.615492	48.382298
1679.947520	95.855599	48.387303
1676.089067	98.967921	48.392308
1672.933485	96.823510	48.397313
1669.269783	103.009109	48.402317
1665.818621	96.858007	48.407322
1662.546580	92.045745	48.412327
1658.512922	107.065023	48.417332
1655.422972	93.002240	48.422337
1651.691721	96.224477	48.427341
1648.388451	92.970453	48.432346
1645.158651	97.111208	48.437351
1641.576728	101.426989	48.442356
1638.110655	93.190172	48.447361
1634.015136	99.828952	48.452365
1630.990490	99.309288	48.457370
1627.733184	97.664761	48.462375
1623.874562	98.309429	48.467380
1620.559523	97.452158	48.472385
1617.345159	94.915113	48.477389
1614.116823	83.705393	48.482394
1610.276009	92.436858	48.487399
1606.828283	98.231345	48.492404
1603.277975	92.045066	48.497409
1599.513530	95.724881	48.502413
1596.079140	103.279473	48.507418
1592.763925	92.004181	48.512423
1589.068141	99.112247	48.517428
1585.880350	88.895947	48.522433
1581.879469	95.763602	48.527437
1578.718782	91.158642	48.532442
1575.425078	87.950594	48.537447
1571.605893	97.184887	48.542452
1568.225537	99.083873	48.547457
1564.963807	97.471678	48.552461
1561.497088	90.943370	48.557466
1558.110784	96.434076	48.562471
1554.258276	91.772285	48.567476
1551.434011	88.374117	48.572481
1547.433603	91.315556	48.577485
1543.734520	98.009693	48.582490
1540.289146	89.662107	48.587495
1536.448073	102.091976	48.592500
1533.394908	87.637527	48.597505
1529.896714	85.536967	48.602509
1526.505729	84.590288	48.607514
1522.586996	84.899480	48.612519
1519.368288	93.673323	48.617524
1516.038759	95.798515	48.622529
1512.170461	97.956946	48.627533
1508.717963	101.895094	48.632538
1505.737024	88.441790	48.637543
1502.211305	96.140308	48.642548
1498.623151	93.705747	48.647553
1495.144855	94.867024	48.652557
1491.035663	99.128842	48.657562
1487.971768	90.218862	48.662567
1484.341980	95.143203	48.667572
1481.109648	81.425323	48.672577
1477.543754	89.164893	48.677581
1473.562762	90.679656	48.682586
1470.312816	90.084345	48.687591
1467.022848	96.256072	48.692596
1463.854575	86.615713	48.697601
1460.078680	85.058248	48.702605
1456.528011	87.249501	48.707610
1453.189282	87.367186	48.712615
1449.874468	87.240709	48.717620
1446.377198	76.642348	48.722625
1442.465815	86.457289	48.727629
1438.805420	79.541543	48.732634
1435.317918	76.544008	48.737639
1431.683171	86.344365	48.742644
1428.364054	79.982930	48.747649
1424.952673	85.635726	48.752653
1421.305669	77.161365	48.757658
1418.155845	85.117743	48.762663
1414.511124	90.012774	48.767668
1411.248131	85.452234	48.772673
1407.898499	78.212883	48.777677
1404.011167	87.565347	48.782682
1400.775255	79.662904	48.787687
1397.011823	85.709012	48.792692
1393.804017	80.497658	48.797697
1390.006586	79.721821	48.802701
1386.419475	87.328657	48.807706
1382.907813	86.112880	48.812711
1379.353475	88.393294	48.817716
1376.221502	89.117870	48.822721
1372.748002	90.022153	48.827725
1369.140264	95.480895	48.832730
1365.727959	86.403708	48.837735
1361.775314	92.517236	48.842740
1358.505584	86.290488	48.847745
1354.841920	91.508003	48.852749
1351.437070	89.570102	48.857754
1347.911980	88.805662	48.862759
1344.564009	91.107741	48.867764
1341.211031	93.182814	48.872769
1337.860856	94.504493	48.877773
1334.178257	92.609825	48.882778
1330.563497	84.143112	48.887783
1327.077142	88.152976	48.892788
1323.400044	91.173823	48.897793
1320.111312	89.243161	48.902797
1316.592610	84.548432	48.907802
1313.359709	88.493537	48.912807
1309.479780	84.908543	48.917812
1306.043865	87.097765	48.922817
1302.543294	91.049733	48.927821
1298.884299	90.233377	48.932826
1295.718637	85.331843	48.937831
1292.121851	88.862200	48.942836
1288.589108	76.991261	48.947841
1285.294676	84.998624	48.952845
1281.434735	83.476409	48.957850
1277.796437	77.816397	48.962855
1274.399091	81.559315	48.967860
1271.229173	84.206998	48.972865
1267.943306	88.150859	48.977869
1264.295991	79.879049	48.982874
1260.138342	76.922573	48.987879
1256.884569	80.421686	48.992884
1253.497877	73.903123	48.997889
1249.946345	77.239779	49.002893
1246.574230	74.135725	49.007898
1243.128605	68.980395	49.012903
1239.419964	78.187990	49.017908
1236.287429	68.817358	49.022913
1232.556230	80.708104	49.027917
1228.972448	80.294491	49.032922
1225.116526	72.874556	49.037927
1221.483733	71.589070	49.042932
1218.493785	66.445072	49.047937
1215.696620	86.669100	49.052941
1211.881900	77.104102	49.057946
1208.388140	75.850759	49.062951
1204.556948	79.243604	49.067956
1201.280386	72.768018	49.072961
1197.349049	77.565307	49.077965
1193.701561	84.681686	49.082970
1190.691399	76.386644	49.087975
1187.166658	83.082129	49.092980
1183.280469	77.011476	49.097985
1180.301430	84.365486	49.102989
1176.197260	81.770848	49.107994
1173.130984	74.591833	49.112999
1169.333983	80.760234	49.118004
1166.133600	82.106067	49.123009
1162.647785	81.626595	49.128013
1159.225023	83.162063	49.133018
1155.405020	75.087994	49.138023
1151.804100	90.131639	49.143028
1148.198184	79.524936	49.148033
1144.855532	77.336940	49.153037
1141.340116	85.938676	49.158042
1138.214559	83.748525	49.163047
1134.747359	82.336035	49.168052
1131.125171	87.214922	49.173057
1127.456027	81.853957	49.178061
1123.938010	85.058861	49.183066
1120.319071	78.225300	49.188071
1117.309509	80.395628	49.193076
1113.474971	76.262610	49.198081
1110.108584	81.329465	49.203085
1106.429753	81.886093	49.208090
1102.922250	77.290893	49.213095
1099.596043	89.814615	49.218100
1095.896355	76.457465	49.223105
1092.918889	86.253593	49.228109
1088.848099	84.644004	49.233114
1085.385600	82.851147	49.238119
1081.931500	86.349818	49.243124
1078.733906	88.334289	49.248129
1074.903081	76.519286	49.253133
1071.166660	72.915156	49.258138
1068.096039	73.310678	49.263143
1064.387692	76.276299	49.268148
1061.028577	77.912599	49.273153
1057.266336	84.679860	49.278157
1053.924112	86.373642	49.283162
1050.740678	83.755922	49.288167
1046.901454	86.789373	49.293172
1043.006607	86.205908	49.298177
1040.145775	82.677454	49.303181
1036.199712	87.015154	49.308186
1033.013558	79.630197	49.313191
1029.390226	79.251238	49.318196
1025.905826	79.802919	49.323201
1022.633029	82.368562	49.328205
1018.904206	84.461037	49.333210
1015.717306	79.116772	49.338215
1011.979987	79.508513	49.343220
1008.167753	72.676588	49.348225
1004.643094	86.009463	49.353229
1001.291611	87.296576	49.358234
998.212584	83.811582	49.363239
994.518613	84.715419	49.368244
990.913677	74.339549	49.373249
987.435061	77.576294	49.378253
983.788310	78.741695	49.383258
980.561346	68.091865	49.388263
976.805779	80.451467	49.393268
973.103798	74.912149	49.398273
970.037931	82.140478	49.403277
966.373158	75.203351	49.408282
963.255637	75.720076	49.413287
959.323158	83.032686	49.418292
956.016583	78.254375	49.423297
952.480559	72.657590	49.428301
948.688727	87.129849	49.433306
945.416794	71.108776	49.438311
942.049400	73.477183	49.443316
938.391323	76.988635	49.448321
934.875116	79.307443	49.453325
931.176460	83.306091	49.458330
928.091179	74.247688	49.463335
923.998416	81.506157	49.468340
920.799207	79.691320	49.473345
917.300660	83.899259	49.478349
913.732611	80.873203	49.483354
910.620971	74.280244	49.488359
906.713298	84.407829	49.493364
903.512814	75.367362	49.498369
899.739464	79.260583	49.503373
896.420339	83.041972	49.508378
892.792630	83.008550	49.513383
889.101707	91.172558	49.518388
885.562505	69.337144	49.523393
882.399832	81.759477	49.528397
878.731866	83.127503	49.533402
875.328384	73.409979	49.538407
871.712757	74.510438	49.543412
868.256059	87.541677	49.548417
864.579456	77.869832	49.553421
861.174882	87.602738	49.558426
858.265892	81.870395	49.563431
854.503913	80.222261	49.568436
850.708234	81.135621	49.573441
847.280096	79.944871	49.578445
843.750673	82.208801	49.583450
840.416361	72.613391	49.588455
836.777448	82.392265	49.593460
833.222435	72.954595	49.598465
829.796748	74.348186	49.603469
826.451387	80.863911	49.608474
822.782936	77.945246	49.613479
818.990891	79.253502	49.618484
815.805109	72.020385	49.623489
812.665355	73.511832	49.628493
808.816229	74.063367	49.633498
805.421604	68.811584	49.638503
801.434576	77.420306	49.643508
798.017287	75.585650	49.648513
794.937624	70.601206	49.653517
791.452460	78.692056	49.658522
787.879771	78.694374	49.663527
784.164464	74.979437	49.668532
780.559368	73.379657	49.673537
777.442543	70.561786	49.678541
773.585626	76.442156	49.683546
770.091597	71.395672	49.688551
766.600439	85.248500	49.693556
763.226320	80.645244	49.698561
759.659419	80.409389	49.703565
755.947834	84.928908	49.708570
753.301935	76.529782	49.713575
749.284301	83.491840	49.718580
745.477135	85.802179	49.723585
742.267151	80.945591	49.728589
738.739602	84.474707	49.733594
735.392785	75.672181	49.738599
731.641569	77.787155	49.743604
728.357502	73.173051	49.748609
724.626420	80.871929	49.753613
720.765954	75.904640	49.758618
717.757442	81.311270	49.763623
714.034212	83.380762	49.768628
710.608009	84.106912	49.773633
707.363629	70.264543	49.778637
703.873241	84.778457	49.783642
700.321021	75.375179	49.788647
696.310047	84.060404	49.793652
692.838829	77.178616	49.798657
689.562981	72.246872	49.803661
686.123053	77.192329	49.808666
682.735657	74.362808	49.813671
679.229576	85.658554	49.818676
675.825876	76.333398	49.823681
672.498747	79.511790	49.828685
668.565314	77.194367	49.833690
664.855995	79.084533	49.838695
661.589521	78.472902	49.843700
657.973067	76.102973	49.848705
654.777217	78.058737	49.853709
650.701036	85.090028	49.858714
647.895725	68.822391	49.863719
644.447933	74.392317	49.868724
640.714514	74.017889	49.873729
637.401479	67.813824	49.878733
633.134086	77.348865	49.883738
629.847024	74.472096	49.888743
626.451778	80.891198	49.893748
623.499217	81.065912	49.898753
619.826977	82.915512	49.903757
616.068213	76.995964	49.908762
612.638440	74.286941	49.913767
608.984274	78.430549	49.918772
605.615373	73.706288	49.923777
601.903282	71.256346	49.928781
598.083805	75.919220	49.933786
594.813803	71.249167	49.938791
591.366308	73.563641	49.943796
588.219688	71.183856	49.948801
584.915731	74.801560	49.953805
581.104135	66.077751	49.958810
577.971042	68.985505	49.963815
573.968458	74.018562	49.968820
570.293558	69.066705	49.973825
566.863606	74.323821	49.978829
563.491398	72.067740	49.983834
560.220580	73.402451	49.988839
556.350423	76.197167	49.993844
553.273054	78.011113	49.998849
549.668777	66.860143	50.003853
545.855083	75.729792	50.008858
542.594762	76.635776	50.013863
539.098003	76.835108	50.018868
535.553155	75.162711	50.023873
532.216214	78.203442	50.028877
528.033661	69.540555	50.033882
525.035709	72.367167	50.038887
521.802271	75.616406	50.043892
518.056515	74.490965	50.048897
514.606294	72.057216	50.053901
511.013885	75.748306	50.058906
507.575494	72.455364	50.063911
504.099176	69.962406	50.068916
500.432636	67.872375	50.073921
497.030588	71.518012	50.078925
492.835514	75.005541	50.083930
489.472788	79.736522	50.088935
486.166238	76.606550	50.093940
483.077440	74.698654	50.098945
479.515114	76.502686	50.103949
476.045751	80.851648	50.108954
472.562617	74.639290	50.113959
469.304273	76.171380	50.118964
466.038001	74.123440	50.123969
461.854497	77.916047	50.128973
458.005955	78.502339	50.133978
455.036528	68.075109	50.138983
451.708106	72.917807	50.143988
448.098489	70.597465	50.148993
444.418103	68.231196	50.153997
440.729939	72.541458	50.159002
437.323665	66.525946	50.164007
433.673239	65.192694	50.169012
430.474983	66.573069	50.174017
426.915576	72.182533	50.179021
423.239902	74.070655	50.184026
419.806852	76.487300	50.189031
416.538592	74.914226	50.194036
413.132202	73.194983	50.199041
409.608700	71.813502	50.204045
405.937360	75.346053	50.209050
402.182185	67.859980	50.214055
398.595466	70.085422	50.219060
395.023059	69.793528	50.224065
392.048726	71.952107	50.229069
388.566686	74.914204	50.234074
384.889675	71.902032	50.239079
381.302202	68.543738	50.244084
377.803255	68.784559	50.249089
374.534263	75.661734	50.254093
370.942708	77.628513	50.259098
367.665796	73.747323	50.264103
363.632083	73.204557	50.269108
360.198367	78.832425	50.274113
356.825712	67.838423	50.279117
353.071256	70.036201	50.284122
350.113520	63.884440	50.289127
346.325483	73.623276	50.294132
342.702047	71.286120	50.299137
339.388506	64.139419	50.304141
335.468865	68.821076	50.309146
332.200596	73.094453	50.314151
329.134854	66.206558	50.319156
325.584786	69.701255	50.324161
322.041571	74.213584	50.329165
318.167141	79.938541	50.334170
315.103988	70.674338	50.339175
311.184344	66.039034	50.344180
307.668327	72.252340	50.349185
304.110995	72.176404	50.354189
300.643180	77.505875	50.359194
297.229292	67.796423	50.364199
293.649307	66.420590	50.369204
290.085238	65.741447	50.374209
287.118389	59.350679	50.379213
283.181838	69.062020	50.384218
279.806289	65.025365	50.389223
276.176168	74.030962	50.394228
272.693100	70.314757	50.399233
269.638294	65.098744	50.404237
265.761154	60.096178	50.409242
262.569302	62.538562	50.414247
259.011361	62.541819	50.419252
254.834619	67.687441	50.424257
251.520633	63.568443	50.429261
247.695647	70.598623	50.434266
244.349039	63.327379	50.439271
241.333846	62.357154	50.444276
238.164991	76.235730	50.449281
234.825422	64.224238	50.454285
230.457928	68.627631	50.459290
227.334390	58.499685	50.464295
223.166135	65.621271	50.469300
219.989853	67.279814	50.474305
216.798315	70.813614	50.479309
213.159108	70.317018	50.484314
209.684104	64.103448	50.489319
206.564639	63.658809	50.494324
202.752373	67.608780	50.499329
198.985529	66.432890	50.504333
195.666488	69.828361	50.509338
192.009777	62.244751	50.514343
188.151337	68.410140	50.519348
185.001317	63.936605	50.524353
181.686219	62.285440	50.529357
178.442476	67.921709	50.534362
174.904755	58.019604	50.539367
171.315060	63.425004	50.544372
167.634322	66.221914	50.549377
164.280213	56.351336	50.554381
160.669266	60.915351	50.559386
157.417180	62.073192	50.564391
153.552630	66.828547	50.569396
150.310000	64.536538	50.574401
146.496970	64.940182	50.579405
143.099271	65.374073	50.584410
139.725544	58.502530	50.589415
136.108669	68.980333	50.594420
132.336115	68.311527	50.599425
129.087411	66.232431	50.604429
125.706015	77.546744	50.609434
122.419352	58.573341	50.614439
118.455573	59.114352	50.619444
114.871835	74.421054	50.624449
111.743404	65.815607	50.629453
107.606326	75.362038	50.634458
105.005231	66.902272	50.639463
101.659716	66.670006	50.644468
97.445769	73.706977	50.649473
93.829681	66.616918	50.654477
90.365992	70.572741	50.659482
86.953886	62.359468	50.664487
83.547831	66.815665	50.669492
79.930131	66.470760	50.674497
76.836247	63.630438	50.679501
73.295394	62.862295	50.684506
69.701092	57.255768	50.689511
66.055314	64.084061	50.694516
62.235019	72.704843	50.699521
58.818726	63.793061	50.704525
55.368057	73.182008	50.709530
52.243726	68.381803	50.714535
48.613630	67.434576	50.719540
44.936618	70.246740	50.724545
41.351479	61.086015	50.729549
37.954171	64.873325	50.734554
34.885179	71.665603	50.739559
30.807811	70.721579	50.744564
27.181638	65.952059	50.749569
24.211302	63.892912	50.754573
20.838220	75.111024	50.759578
17.674378	63.255717	50.764583
13.580772	65.952419	50.769588
9.477241	63.607815	50.774593
6.552158	64.784361	50.779597
2.951106	65.746626	50.784602