Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3927_Position 121_00000.hld	3008.298458	439217.248571	669.857392	226515750.101913	3522.594444	3500.064228	39.433741	1.939014	0.000000	-262.920454	5.738989	-129.943000	-51.863500	0.241896
3927_Position 121_00001.hld	3027.195850	426686.065394	673.091953	229333108.004930	3520.935578	3502.635421	39.380012	1.860552	0.000000	-146.629696	5.756670	-129.893000	-51.863500	0.021600
3927_Position 121_00002.hld	3019.326084	446989.319764	701.221833	228157704.572817	3520.945327	3497.408731	41.131324	1.959124	0.000000	-173.976553	5.759546	-129.843000	-51.863500	0.008164
3927_Position 121_00003.hld	3027.368060	434785.761697	689.641868	229358862.671706	3520.494766	3500.206698	40.346019	1.895657	0.000000	-131.700067	5.760803	-129.793000	-51.863500	-0.047382
3927_Position 121_00004.hld	3030.729292	444179.177884	712.950388	229861837.180994	3520.592528	3497.990954	41.663975	1.932375	0.000000	-98.551525	5.772797	-129.743000	-51.863500	-0.044196
3927_Position 121_00005.hld	3040.800136	461184.350491	756.812361	231372146.371328	3520.863050	3497.833188	44.082631	1.993258	0.000000	-30.163922	5.789511	-129.943000	-51.813500	-0.047081
3927_Position 121_00006.hld	3049.808262	463389.948617	778.304028	232727284.947658	3520.976067	3496.346439	45.202292	1.991129	0.000000	-5.271973	5.881275	-129.893000	-51.813500	-0.042891
3927_Position 121_00007.hld	3051.472632	471785.301515	797.775119	232978099.140558	3520.045704	3495.004861	46.308186	2.025020	0.000000	-4.809348	5.918083	-129.843000	-51.813500	-0.021332
3927_Position 121_00008.hld	3045.120948	490770.796861	826.413787	232021652.826767	3520.522920	3490.512957	48.069336	2.115194	0.000000	-2.488729	5.881900	-129.793000	-51.813500	-0.047540
3927_Position 121_00009.hld	3063.890822	468556.454068	814.884688	234853749.879907	3519.953796	3495.138759	47.112075	1.995099	0.000000	-4.976941	6.087187	-129.743000	-51.813500	-0.014926
3927_Position 121_00010.hld	3066.956514	490577.282028	865.194923	235317954.921548	3520.965406	3492.216709	49.971370	2.084742	0.000000	-3.333804	6.164844	-129.943000	-51.763500	-0.021971
3927_Position 121_00011.hld	3087.871173	463080.734565	848.407490	238497105.554412	3519.845901	3497.238788	48.674082	1.941662	0.000000	-6.369539	6.418940	-129.893000	-51.763500	-0.036044
3927_Position 121_00012.hld	3088.618371	471060.836446	866.454131	238611079.915249	3520.172228	3496.367165	49.697564	1.974178	0.000000	-5.221133	6.440709	-129.843000	-51.763500	-0.027653
3927_Position 121_00013.hld	3085.932712	485687.310160	895.983146	238201548.432566	3519.629360	3492.486657	51.435430	2.038976	0.000000	-3.655547	6.449591	-129.793000	-51.763500	0.032641
3927_Position 121_00014.hld	3094.428966	481389.089681	909.603635	239498335.078098	3519.044280	3491.351102	52.075778	2.009989	0.000000	-3.419869	6.603507	-129.743000	-51.763500	0.030058
3927_Position 121_00015.hld	3087.642644	507094.226120	945.198549	238462252.146340	3519.254306	3490.013839	54.231055	2.126518	0.000000	-2.308391	6.509516	-129.943000	-51.713500	-0.029259
3927_Position 121_00016.hld	3088.585369	517912.546828	969.829608	238606045.371312	3520.460946	3489.103571	55.627500	2.170576	0.000000	-1.224590	6.535898	-129.893000	-51.713500	0.011610
3927_Position 121_00017.hld	3101.243374	504694.650512	972.863324	240540972.704706	3520.484370	3490.322681	55.576620	2.098165	0.000000	-2.007163	6.731911	-129.843000	-51.713500	0.027837
3927_Position 121_00018.hld	3114.353496	475500.031260	936.719436	242553274.673563	3519.218118	3495.070507	53.289395	1.960394	0.000000	-4.882591	6.894793	-129.793000	-51.713500	0.038618
3927_Position 121_00019.hld	3098.672472	524035.316554	1013.482716	240147345.382185	3520.053635	3486.470390	57.944508	2.182141	0.000000	-0.085413	6.742988	-129.743000	-51.713500	0.036902
3927_Position 121_00020.hld	3099.494054	529827.240892	1026.188144	240273101.580282	3519.734898	3486.723660	58.655568	2.205104	0.000000	110.566305	6.539061	-129.943000	-51.663500	0.013392
3927_Position 121_00021.hld	3109.572609	517189.485577	1022.544740	241818471.644415	3520.202682	3488.912602	58.260259	2.138751	0.000000	-1.572105	6.901101	-129.893000	-51.663500	0.040365
3927_Position 121_00022.hld	3101.205989	529517.066756	1030.093356	240535246.537864	3518.904835	3486.741725	58.846692	2.201412	0.000000	402.504458	5.999905	-129.843000	-51.663500	0.041438
3927_Position 121_00023.hld	3115.211233	521767.626054	1052.436658	242685223.749580	3519.213290	3487.039520	59.856198	2.149977	0.000000	-0.602754	7.034784	-129.793000	-51.663500	0.034884
3927_Position 121_00024.hld	3116.600211	521558.011015	1056.776491	242898971.916651	3518.065979	3486.752756	60.076571	2.147222	0.000000	-0.505826	7.065854	-129.743000	-51.663500	0.047759