Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
Forged_00000.hld	2768.535217	402160.699117	406.427941	205045151.313028	3522.788503	3510.660682	25.147431	1.961328	42.126907	2241.728127	1.282397	-134.943000	-66.358500	-0.173117
Forged_00001.hld	2703.429812	436634.121714	404.258753	195762027.922627	3522.820560	3513.494130	25.599415	2.230433	54.213332	2165.492590	1.248050	-134.893000	-66.358500	-0.141516
Forged_00002.hld	2696.062923	440219.216238	404.068283	194724933.024231	3522.204507	3513.163463	25.655401	2.260723	49.476395	2141.680866	1.258856	-134.843000	-66.358500	-0.134687
Forged_00003.hld	2697.356247	439808.239649	404.206326	194906808.427438	3521.747490	3513.415173	25.652189	2.256505	49.982163	2144.937952	1.257701	-134.793000	-66.358500	-0.104918
Forged_00004.hld	2686.120209	447128.262642	404.924494	193329513.937738	3521.712160	3514.289910	25.802382	2.312778	48.800154	2122.566405	1.260361	-134.743000	-66.358500	-0.064813
Forged_00005.hld	2718.034038	439226.067970	414.450506	197825986.451888	3520.883456	3512.868514	26.107533	2.220265	50.064407	2176.081797	1.261382	-134.943000	-66.308500	-0.048691
Forged_00006.hld	2690.683787	454976.072737	414.444978	193969380.705323	3521.532856	3514.030847	26.365446	2.345608	53.337993	2138.970007	1.252565	-134.893000	-66.308500	-0.047124
Forged_00007.hld	2699.031802	449052.526172	413.604523	195142559.682631	3521.520025	3513.310603	26.232767	2.301151	48.438667	2140.566960	1.264380	-134.843000	-66.308500	-0.034588
Forged_00008.hld	2710.661569	443420.812464	414.126790	196782733.733719	3520.569895	3513.714202	26.156201	2.253352	56.982429	2180.456024	1.245178	-134.793000	-66.308500	-0.049791
Forged_00009.hld	2702.164025	442906.001910	409.372258	195583640.412704	3519.909165	3513.600303	25.935043	2.264535	62.070026	2179.565019	1.233031	-134.743000	-66.308500	-0.034666
Forged_00010.hld	2717.988704	451077.704865	424.907894	197819563.088993	3522.441516	3514.180734	26.766711	2.280248	53.649973	2180.899219	1.255930	-134.943000	-66.258500	-0.043660
Forged_00011.hld	2685.985894	466642.138032	421.383381	193310697.161960	3522.509771	3516.539778	26.852473	2.413949	55.738223	2133.426186	1.248968	-134.893000	-66.258500	-0.036849
Forged_00012.hld	2730.309604	441960.877742	423.399127	199569077.661943	3520.497206	3513.189486	26.554502	2.214576	52.409154	2199.117273	1.258883	-134.843000	-66.258500	-0.035709
Forged_00013.hld	2765.307909	420767.692086	422.880452	204580000.513578	3520.872921	3511.560821	26.195148	2.056739	57.736867	2269.449667	1.248348	-134.793000	-66.258500	-0.038964
Forged_00014.hld	2695.921997	458160.192377	419.805998	194705120.097875	3521.383374	3514.443279	26.655988	2.353098	56.907505	2154.140627	1.246427	-134.743000	-66.258500	-0.002931
Forged_00015.hld	2727.004320	454187.003210	433.126884	199098998.123543	3520.909264	3513.471901	27.196651	2.281212	53.849561	2194.092720	1.258201	-134.943000	-66.208500	-0.034361
Forged_00016.hld	2718.369872	455818.177229	429.676968	197873573.792356	3520.452849	3513.999283	27.063440	2.303583	51.774513	2175.586934	1.261654	-134.893000	-66.208500	-0.018898
Forged_00017.hld	2783.916405	419955.813935	433.150390	207269175.318578	3521.152872	3511.069993	26.656687	2.026137	55.918856	2293.278104	1.256054	-134.843000	-66.208500	-0.035464
Forged_00018.hld	2766.238930	425471.151774	428.477481	204714134.843662	3520.259314	3510.976699	26.533156	2.078367	58.062517	2270.405943	1.249336	-134.793000	-66.208500	-0.021575
Forged_00019.hld	2734.779990	446760.235799	430.210977	200205725.843959	3520.747160	3513.630821	26.938789	2.231506	56.525278	2213.730488	1.251748	-134.743000	-66.208500	0.011819
Forged_00020.hld	2718.484287	469642.067887	442.311542	197889787.534516	3520.851290	3514.826948	27.858095	2.373251	54.519724	2178.182718	1.258859	-134.943000	-66.158500	-0.044223
Forged_00021.hld	2749.315984	449572.003780	441.584394	202282755.997497	3520.989957	3512.882378	27.508640	2.222493	59.560797	2241.143619	1.249144	-134.893000	-66.158500	-0.042268
Forged_00022.hld	2789.431769	421986.051362	438.854797	208069536.950140	3522.664326	3510.603192	26.955750	2.028101	61.467593	2312.265286	1.246241	-134.843000	-66.158500	-0.042632
Forged_00023.hld	2794.084679	419216.953319	438.294415	208745923.605575	3521.256726	3511.439736	26.877679	2.008264	61.032688	2318.599768	1.247123	-134.793000	-66.158500	-0.007508
Forged_00024.hld	2783.858193	426680.198608	439.549431	207260736.096430	3520.525940	3511.899516	27.051044	2.058664	64.452754	2307.922661	1.240290	-134.743000	-66.158500	-0.045843