Fri Mar 05 17:47:13 2021

Number of Points = 14581

Depth (nm)	Load (N)	Time (s)
-0.220132	107.730986	0.000000
-0.471467	94.296991	0.005005
-1.338223	64.982659	0.010010
-3.098791	19.037671	0.015014
-6.555538	-21.951286	0.020019
-12.006677	-18.615214	0.025024
-17.114086	-27.970647	0.030029
-22.250570	-17.690644	0.035034
-26.276608	-25.553212	0.040038
-29.998024	-20.406610	0.045043
-33.610556	-17.019981	0.050048
-37.002098	-25.911031	0.055053
-40.808888	-18.194440	0.060058
-44.318544	-17.076196	0.065062
-48.020594	-29.406070	0.070067
-51.994547	-14.974643	0.075072
-55.740189	-17.751833	0.080077
-59.910619	-12.818998	0.085082
-63.773496	-13.011657	0.090086
-67.189127	-13.897006	0.095091
-70.894104	-9.725987	0.100096
-74.439752	-15.875190	0.105101
-78.473885	-11.585414	0.110106
-82.107107	-11.937689	0.115110
-85.513016	-19.441752	0.120115
-89.985424	-9.985098	0.125120
-93.024408	-21.190611	0.130125
-97.387305	-19.237544	0.135130
-101.048300	-13.778762	0.140134
-104.615679	-22.840364	0.145139
-108.774547	-8.451887	0.150144
-112.569316	-18.360333	0.155149
-116.115316	-14.908502	0.160154
-119.352902	-13.190133	0.165158
-123.452762	-17.153395	0.170163
-127.410439	-17.857553	0.175168
-131.116590	-20.516340	0.180173
-134.545894	-15.386227	0.185178
-138.379986	-15.223799	0.190182
-142.301470	-25.665506	0.195187
-146.504208	-19.574570	0.200192
-149.964949	-25.464376	0.205197
-153.861135	-16.949573	0.210202
-157.860852	-24.186879	0.215206
-161.372921	-20.975375	0.220211
-165.173512	-13.645956	0.225216
-168.665355	-25.982366	0.230221
-172.880965	-16.421463	0.235226
-176.452430	-17.641350	0.240230
-180.146704	-12.804797	0.245235
-183.732410	-21.770306	0.250240
-187.208935	-20.802230	0.255245
-191.040162	-12.837075	0.260250
-195.109972	-25.710442	0.265254
-198.875442	-23.267458	0.270259
-202.734513	-20.729103	0.275264
-206.180385	-27.214157	0.280269
-209.979001	-14.792789	0.285274
-213.992876	-7.916557	0.290278
-217.430916	-8.559987	0.295283
-221.452086	-7.564867	0.300288
-225.313864	-15.980031	0.305293
-228.992118	-21.048073	0.310298
-232.545370	-20.468249	0.315302
-236.136543	-26.430153	0.320307
-240.308776	-22.652686	0.325312
-243.551276	-18.831202	0.330317
-247.638325	-13.036114	0.335322
-251.785272	-18.663279	0.340326
-255.303120	-22.712893	0.345331
-259.360000	-13.989346	0.350336
-262.990205	-21.384800	0.355341
-266.733563	-17.499114	0.360346
-270.271173	-14.442656	0.365350
-274.078289	-22.161530	0.370355
-277.811807	-15.454533	0.375360
-281.387548	-21.997597	0.380365
-285.290686	-16.914654	0.385370
-288.977589	-18.713637	0.390374
-292.635837	-19.389620	0.395379
-296.673410	-17.249996	0.400384
-300.622027	-15.324845	0.405389
-304.608403	-22.586105	0.410394
-307.985270	-8.839407	0.415398
-311.327512	-17.838848	0.420403
-315.318920	-15.758603	0.425408
-319.069205	-21.352768	0.430413
-323.279207	-16.840547	0.435418
-327.172385	-7.742459	0.440422
-330.621109	-16.149262	0.445427
-334.524248	-10.124759	0.450432
-337.783641	-16.696161	0.455437
-341.475075	-18.065391	0.460442
-345.237116	-13.362861	0.465446
-349.338246	-12.345301	0.470451
-353.182142	-16.382143	0.475456
-356.958340	-23.003478	0.480461
-360.807609	-13.636374	0.485466
-364.392631	-22.469234	0.490470
-367.788564	-24.377628	0.495475
-371.820826	-14.525534	0.500480
-375.622441	-18.800911	0.505485
-379.630712	-12.904639	0.510490
-383.188956	-19.650621	0.515494
-387.090001	-21.864711	0.520499
-390.895650	-14.441102	0.525504
-394.219572	-28.338400	0.530509
-398.164961	-17.082399	0.535514
-402.044314	-21.931970	0.540518
-405.674576	-20.901184	0.545523
-409.788135	-20.411415	0.550528
-413.334787	-21.327390	0.555533
-417.179854	-10.938964	0.560538
-420.648749	-19.742968	0.565542
-424.534161	-14.419775	0.570547
-428.287686	-14.146742	0.575552
-431.898667	-21.538688	0.580557
-435.710983	-20.551329	0.585562
-439.471983	-18.326316	0.590566
-443.162563	-21.651023	0.595571
-447.346697	-19.617060	0.600576
-450.736279	-29.176452	0.605581
-454.750440	-30.639053	0.610586
-458.578347	-24.738343	0.615590
-462.316198	-20.898974	0.620595
-466.162664	-21.027372	0.625600
-469.688481	-19.219930	0.630605
-473.068765	-17.377374	0.635610
-476.991199	-21.360465	0.640614
-480.940074	-23.275013	0.645619
-484.981585	-16.387630	0.650624
-488.810226	-26.523423	0.655629
-492.489679	-24.932696	0.660634
-496.017437	-27.743982	0.665638
-499.470945	-29.657183	0.670643
-503.868743	-18.800296	0.675648
-507.258251	-25.052614	0.680653
-511.221746	-24.375318	0.685658
-514.889076	-16.825376	0.690662
-518.480761	-25.265824	0.695667
-522.394076	-18.876692	0.700672
-526.055444	-21.122524	0.705677
-529.799331	-20.030823	0.710682
-533.721819	-17.699443	0.715686
-537.267083	-29.244530	0.720691
-541.445270	-13.270547	0.725696
-544.959663	-23.281391	0.730701
-548.786055	-14.509038	0.735706
-552.276708	-20.816101	0.740710
-555.823034	-20.153323	0.745715
-560.006659	-18.434650	0.750720
-563.713864	-21.021621	0.755725
-567.656411	-16.304113	0.760730
-571.390650	-15.746920	0.765734
-574.973347	-25.637989	0.770739
-579.111819	-15.137797	0.775744
-582.652925	-17.604610	0.780749
-586.651597	-15.571645	0.785754
-590.023568	-16.887436	0.790758
-593.867520	-17.672067	0.795763
-597.572429	-11.226216	0.800768
-600.984019	-18.515699	0.805773
-605.077815	-22.813410	0.810778
-608.785652	-20.065173	0.815782
-612.521432	-12.952023	0.820787
-616.638762	-13.029021	0.825792
-620.184376	-19.439167	0.830797
-623.834518	-13.686452	0.835802
-627.700036	-13.510335	0.840806
-631.563058	-19.402958	0.845811
-635.052774	-18.897347	0.850816
-638.972915	-24.001785	0.855821
-643.108552	-17.223692	0.860826
-646.797908	-26.104085	0.865830
-650.318191	-24.169526	0.870835
-654.314643	-10.101042	0.875840
-657.286441	-24.931014	0.880845
-661.433764	-11.872935	0.885850
-665.350018	-15.530254	0.890854
-668.928733	-21.438276	0.895859
-672.909593	-16.618279	0.900864
-676.697217	-25.326798	0.905869
-680.347013	-17.730529	0.910874
-684.243618	-23.261290	0.915878
-687.510249	-27.973307	0.920883
-691.720113	-18.284725	0.925888
-695.489070	-17.579859	0.930893
-699.329650	-17.588967	0.935898
-702.884533	-16.415228	0.940902
-706.465284	-18.921251	0.945907
-710.673238	-16.126058	0.950912
-714.212239	-22.574961	0.955917
-718.277964	-17.370732	0.960922
-721.747887	-24.939299	0.965926
-725.322352	-26.359735	0.970931
-729.667933	-10.748223	0.975936
-733.202809	-20.213003	0.980941
-736.795518	-20.551832	0.985946
-740.117629	-26.467628	0.990950
-743.890662	-18.712796	0.995955
-748.128986	-14.780390	1.000960
-751.737369	-16.554925	1.005965
-755.739805	-12.109827	1.010970
-759.493481	-19.491059	1.015974
-763.093303	-22.705177	1.020979
-766.789880	-16.769782	1.025984
-770.444771	-24.695080	1.030989
-774.516218	-22.929303	1.035994
-777.887431	-13.191677	1.040998
-782.010990	-18.105660	1.046003
-785.966218	-18.686105	1.051008
-789.574752	-23.567266	1.056013
-793.212379	-16.154132	1.061018
-797.093193	-9.829684	1.066022
-800.739937	-16.535632	1.071027
-804.727863	-13.387498	1.076032
-808.434101	-18.055888	1.081037
-812.205437	-16.039960	1.086042
-815.692452	-23.417986	1.091046
-819.156604	-14.944406	1.096051
-823.355276	-12.147345	1.101056
-827.304898	-14.417595	1.106061
-830.853043	-8.378088	1.111066
-834.647707	-14.245024	1.116070
-838.021275	-24.385146	1.121075
-841.990469	-15.974311	1.126080
-845.815116	-20.122223	1.131085
-849.379487	-20.660958	1.136090
-853.459000	-21.372814	1.141094
-857.303348	-27.081948	1.146099
-861.276451	-18.000230	1.151104
-864.625213	-27.854104	1.156109
-868.415705	-17.685046	1.161114
-872.390003	-22.241090	1.166118
-875.442223	-30.467569	1.171123
-879.690150	-16.587208	1.176128
-883.467268	-19.883185	1.181133
-887.257916	-17.241133	1.186138
-891.071370	-26.520764	1.191142
-894.495601	-25.191003	1.196147
-898.962413	-11.327653	1.201152
-902.270308	-19.043276	1.206157
-906.276393	-18.054149	1.211162
-909.994028	-14.587919	1.216166
-913.555147	-17.399546	1.221171
-917.091402	-16.013992	1.226176
-921.009903	-24.328996	1.231181
-924.668938	-16.984790	1.236186
-928.715446	-18.737886	1.241190
-932.225489	-18.408366	1.246195
-936.285153	-15.822574	1.251200
-939.827552	-16.462459	1.256205
-943.751950	-11.124325	1.261210
-947.259099	-17.019695	1.266214
-951.182342	-17.999227	1.271219
-954.976827	-20.057513	1.276224
-958.591227	-28.600852	1.281229
-962.596841	-7.301428	1.286234
-966.585406	-15.329177	1.291238
-969.620811	-19.924794	1.296243
-973.834559	-16.393327	1.301248
-977.162502	-21.511454	1.306253
-981.002847	-14.262754	1.311258
-985.055410	-22.584594	1.316262
-988.746437	-21.686711	1.321267
-992.767554	-19.646323	1.326272
-996.146609	-21.395647	1.331277
-1000.062980	-20.742417	1.336282
-1003.939548	-23.806241	1.341286
-1007.867393	-22.580286	1.346291
-1011.500021	-13.537007	1.351296
-1014.996102	-18.713348	1.356301
-1018.781394	-17.163231	1.361306
-1022.970604	-16.516793	1.366310
-1026.548874	-14.402087	1.371315
-1030.451499	-6.212911	1.376320
-1033.606095	-17.989994	1.381325
-1037.592528	-18.582369	1.386330
-1041.154445	-21.018342	1.391334
-1045.162910	-29.560016	1.396339
-1049.347885	-15.650017	1.401344
-1052.860756	-12.228931	1.406349
-1056.550909	-13.411152	1.411354
-1060.261559	-16.474611	1.416358
-1063.807447	-29.996302	1.421363
-1067.546070	-16.100893	1.426368
-1071.514713	-11.424126	1.431373
-1075.794615	-8.055367	1.436378
-1079.563861	-8.518402	1.441382
-1082.637035	-14.386779	1.446387
-1086.414999	-16.045355	1.451392
-1090.257673	-19.981808	1.456397
-1094.159672	-12.287814	1.461402
-1097.847599	-7.707947	1.466406
-1101.634890	-17.842987	1.471411
-1105.417897	-15.920924	1.476416
-1108.817133	-16.952472	1.481421
-1113.113612	-18.455517	1.486426
-1117.025982	-11.157232	1.491430
-1120.505749	-20.806827	1.496435
-1124.166470	-12.203604	1.501440
-1127.824993	-12.898745	1.506445
-1131.658769	-13.750354	1.511450
-1135.600358	-25.035515	1.516454
-1139.557915	-19.294356	1.521459
-1142.955061	-11.105444	1.526464
-1146.635985	-18.701097	1.531469
-1150.562150	-13.464851	1.536474
-1154.406940	-11.304159	1.541478
-1157.760738	-9.409676	1.546483
-1162.141657	-11.559886	1.551488
-1165.536912	-16.361028	1.556493
-1169.209695	-13.269013	1.561498
-1173.184589	-13.990739	1.566502
-1176.538400	-16.235863	1.571507
-1180.438026	-6.969836	1.576512
-1184.097791	-14.387459	1.581517
-1188.520305	-8.488243	1.586522
-1192.380645	-20.237327	1.591526
-1195.693308	-21.621654	1.596531
-1199.654561	-9.937655	1.601536
-1203.244396	-19.629432	1.606541
-1207.084540	-16.005940	1.611546
-1210.596723	-20.602215	1.616550
-1214.059651	-23.774447	1.621555
-1218.231908	-18.416711	1.626560
-1221.884190	-17.177719	1.631565
-1225.820117	-25.509894	1.636570
-1229.677162	-23.413354	1.641574
-1233.799083	-22.554947	1.646579
-1237.206677	-15.587989	1.651584
-1240.656386	-26.686731	1.656589
-1244.282754	-22.129109	1.661594
-1248.128473	-16.771533	1.666598
-1251.991666	-20.258136	1.671603
-1256.054685	-16.991572	1.676608
-1259.629381	-14.187935	1.681613
-1263.599521	-17.881338	1.686618
-1267.143071	-24.011658	1.691622
-1270.530209	-28.342411	1.696627
-1274.928157	-3.768958	1.701632
-1278.313044	-19.766728	1.706637
-1282.270479	-11.241944	1.711642
-1285.986659	-13.217595	1.716646
-1289.474819	-17.905905	1.721651
-1293.371738	-8.783642	1.726656
-1297.095723	-20.469202	1.731661
-1301.184339	-14.186390	1.736666
-1305.131947	-21.931488	1.741670
-1308.206016	-29.294399	1.746675
-1312.007211	-16.317473	1.751680
-1316.275340	-21.141108	1.756685
-1319.892676	-13.579052	1.761690
-1323.565426	-18.538970	1.766694
-1327.045105	-23.517168	1.771699
-1331.007138	-6.974096	1.776704
-1334.524679	-14.213954	1.781709
-1338.900797	-14.511617	1.786714
-1342.519945	-10.574760	1.791718
-1345.946765	-21.476720	1.796723
-1350.283294	-9.006993	1.801728
-1353.635284	-10.673389	1.806733
-1357.635505	-10.848255	1.811738
-1361.318735	-17.854958	1.816742
-1364.621326	-16.889346	1.821747
-1368.844133	-13.128639	1.826752
-1372.320505	-18.804331	1.831757
-1376.301745	-7.723997	1.836762
-1379.806605	-20.061098	1.841766
-1383.831068	-16.500856	1.846771
-1387.552134	-6.605477	1.851776
-1390.967040	-14.164459	1.856781
-1394.894039	-13.478900	1.861786
-1398.681873	-11.962457	1.866790
-1402.328047	-14.639852	1.871795
-1406.542957	-16.067094	1.876800
-1409.931775	-23.263565	1.881805
-1413.988077	-18.922291	1.886810
-1417.653479	-26.027947	1.891814
-1421.041116	-22.342509	1.896819
-1425.291492	-10.655233	1.901824
-1428.745470	-13.707142	1.906829
-1432.769966	-21.205516	1.911834
-1436.518671	-22.273669	1.916838
-1439.917409	-24.230503	1.921843
-1443.993325	-18.056720	1.926848
-1447.318715	-22.078539	1.931853
-1451.326113	-20.375464	1.936858
-1455.131066	-16.045978	1.941862
-1458.936758	-25.087734	1.946867
-1463.152614	-13.692147	1.951872
-1466.182640	-22.145288	1.956877
-1470.231738	-19.897747	1.961882
-1474.270385	-16.185264	1.966886
-1477.890755	-22.913244	1.971891
-1481.643419	-13.526769	1.976896
-1484.866151	-21.327689	1.981901
-1489.107866	-24.429988	1.986906
-1493.035538	-19.364833	1.991910
-1496.404958	-18.255864	1.996915
-1500.607527	-21.694251	2.006912
-1501.490102	-17.825407	2.016909
-1499.037539	-19.269529	2.026906
-1496.177483	-19.120932	2.036902
-1493.745741	-23.112615	2.046899
-1491.617479	-27.151228	2.056896
-1490.229878	-18.408315	2.066893
-1488.428516	-20.030792	2.076890
-1486.211918	-19.547031	2.086886
-1484.472125	-15.873097	2.096883
-1482.297968	-19.486402	2.106880
-1480.508264	-26.517506	2.116877
-1479.001576	-19.416884	2.126874
-1476.837198	-26.422713	2.136870
-1474.839737	-27.593400	2.146867
-1472.957032	-26.121386	2.156864
-1471.463422	-22.315651	2.166861
-1469.328031	-28.028354	2.176858
-1467.316956	-25.178670	2.186854
-1465.477255	-29.343958	2.196851
-1463.480999	-29.642825	2.206848
-1461.701572	-29.269050	2.216845
-1459.824872	-23.299812	2.226842
-1458.055383	-23.696582	2.236838
-1455.848547	-25.974509	2.246835
-1454.469233	-27.333585	2.256832
-1452.250159	-32.151736	2.266829
-1450.246372	-30.088010	2.276826
-1448.625582	-22.792469	2.286822
-1446.469844	-26.941236	2.296819
-1444.649913	-28.839822	2.306816
-1443.132586	-31.098132	2.316813
-1440.973293	-30.702262	2.326810
-1438.888830	-25.783948	2.336806
-1437.226648	-30.810568	2.346803
-1435.704843	-22.585707	2.356800
-1433.580728	-21.322844	2.366797
-1431.437749	-19.216645	2.376794
-1429.574727	-23.665917	2.386790
-1427.835836	-27.245801	2.396787
-1425.865089	-23.495109	2.406784
-1424.070971	-23.780528	2.416781
-1422.125190	-21.277996	2.426778
-1420.205896	-20.212865	2.436774
-1418.239377	-24.565008	2.446771
-1416.377854	-21.556328	2.456768
-1414.844657	-21.646802	2.466765
-1413.211707	-19.853686	2.476762
-1410.900123	-20.545638	2.486758
-1408.727084	-25.462965	2.496755
-1407.010410	-21.880011	2.506752
-1405.198207	-21.012469	2.516749
-1403.503043	-21.488881	2.526746
-1401.530853	-23.028109	2.536742
-1399.337605	-17.928213	2.546739
-1397.666038	-21.705729	2.556736
-1395.782267	-27.468881	2.566733
-1394.076043	-22.478917	2.576730
-1392.223323	-25.186433	2.586726
-1390.209416	-22.337921	2.596723
-1388.560538	-27.060788	2.606720
-1386.501061	-20.939947	2.616717
-1384.562829	-22.048968	2.626714
-1382.442313	-22.615564	2.636710
-1380.701004	-26.438970	2.646707
-1378.876405	-21.750588	2.656704
-1377.235665	-24.942076	2.666701
-1375.337212	-20.663426	2.676698
-1373.347355	-25.049271	2.686694
-1371.344236	-26.219196	2.696691
-1369.352728	-21.993334	2.706688
-1367.804922	-17.652230	2.716685
-1366.063434	-23.896292	2.726682
-1364.005342	-24.923425	2.736678
-1361.972784	-22.722113	2.746675
-1360.217036	-19.840145	2.756672
-1358.388932	-21.244161	2.766669
-1356.134830	-22.732157	2.776666
-1354.299031	-22.236263	2.786662
-1352.679921	-19.119249	2.796659
-1350.735260	-20.620868	2.806656
-1348.996771	-23.194797	2.816653
-1347.049439	-18.862364	2.826650
-1345.034136	-20.725828	2.836646
-1343.199451	-20.750824	2.846643
-1341.587428	-15.254663	2.856640
-1339.434128	-21.551992	2.866637
-1337.676065	-16.808711	2.876634
-1335.820482	-20.170356	2.886630
-1333.938939	-18.732777	2.896627
-1331.952602	-16.813000	2.906624
-1330.062660	-15.766779	2.916621
-1328.280067	-18.600396	2.926618
-1326.219236	-21.634870	2.936614
-1324.358079	-20.940896	2.946611
-1322.811894	-21.893954	2.956608
-1320.946502	-17.742601	2.966605
-1319.007330	-17.549027	2.976602
-1316.911280	-14.923605	2.986598
-1314.911018	-19.003160	2.996595
-1313.137552	-19.940481	3.006592
-1311.406233	-14.553395	3.016589
-1309.600350	-14.310057	3.026586
-1307.484659	-20.385014	3.036582
-1305.572455	-23.124090	3.046579
-1303.818671	-17.318995	3.056576
-1301.984902	-17.512767	3.066573
-1299.977813	-24.235102	3.076570
-1298.053142	-23.641276	3.086566
-1296.407637	-30.037302	3.096563
-1294.597341	-22.684334	3.106560
-1292.771729	-16.445443	3.116557
-1290.543555	-14.883295	3.126554
-1288.783075	-21.362461	3.136550
-1287.123290	-21.035721	3.146547
-1285.311953	-21.187993	3.156544
-1283.043716	-26.219922	3.166541
-1281.130187	-20.614069	3.176538
-1279.623380	-18.701190	3.186534
-1277.485922	-11.675309	3.196531
-1275.455737	-20.954600	3.206528
-1273.914591	-19.506708	3.216525
-1271.732154	-19.219388	3.226522
-1269.893574	-18.657553	3.236518
-1268.654290	-18.029809	3.246515
-1266.156402	-18.887228	3.256512
-1264.170417	-16.070451	3.266509
-1262.865108	-19.814527	3.276506
-1260.926530	-13.716849	3.286502
-1258.766460	-15.969740	3.296499
-1256.777924	-19.295757	3.306496
-1255.093399	-12.934775	3.316493
-1253.079880	-9.909225	3.326490
-1251.124004	-15.090099	3.336486
-1249.364153	-17.349992	3.346483
-1247.431230	-15.855823	3.356480
-1245.619492	-15.768117	3.366477
-1244.057828	-20.355349	3.376474
-1242.022492	-15.806368	3.386470
-1239.892734	-17.001184	3.396467
-1238.220100	-13.123666	3.406464
-1236.241104	-17.449239	3.416461
-1234.403646	-18.095148	3.426458
-1232.530076	-6.004124	3.436454
-1230.654754	-12.458996	3.446451
-1228.729217	-15.282255	3.456448
-1226.765444	-17.159480	3.466445
-1225.043299	-14.494668	3.476442
-1223.068070	-10.354490	3.486438
-1221.162761	-13.003972	3.496435
-1219.780704	-13.468046	3.506432
-1217.578248	-9.023153	3.516429
-1215.422574	-13.321716	3.526426
-1213.728755	-11.640830	3.536422
-1211.881796	-16.388963	3.546419
-1210.205652	-19.731274	3.556416
-1208.038448	-14.342794	3.566413
-1206.108116	-11.660750	3.576410
-1204.356644	-23.587622	3.586406
-1202.460743	-17.694653	3.596403
-1200.566011	-18.569183	3.606400
-1198.821972	-19.121165	3.616397
-1196.821507	-24.408606	3.626394
-1194.722950	-12.753044	3.636390
-1193.146285	-14.615674	3.646387
-1191.404705	-18.645843	3.656384
-1189.474718	-16.290588	3.666381
-1187.689724	-13.683174	3.676378
-1185.429133	-21.694987	3.686374
-1183.387419	-16.821693	3.696371
-1181.794787	-24.273451	3.706368
-1180.112411	-21.752250	3.716365
-1178.404401	-16.345537	3.726362
-1176.296211	-16.377843	3.736358
-1174.358627	-22.736837	3.746355
-1172.341863	-17.810592	3.756352
-1170.380755	-21.706913	3.766349
-1168.883303	-14.693798	3.776346
-1167.294643	-17.082566	3.786342
-1164.905926	-11.432625	3.796339
-1162.937768	-14.802676	3.806336
-1161.092496	-15.896641	3.816333
-1159.398891	-15.262574	3.826330
-1157.443739	-13.517662	3.836326
-1155.524548	-21.015334	3.846323
-1153.471142	-9.837262	3.856320
-1151.878819	-10.131242	3.866317
-1150.095861	-8.557732	3.876314
-1147.932097	-19.727860	3.886310
-1146.187880	-15.793826	3.896307
-1144.269457	-21.876561	3.906304
-1142.535641	-21.732096	3.916301
-1140.752859	-14.789872	3.926298
-1138.555252	-18.125554	3.936294
-1136.813142	-20.619380	3.946291
-1134.602973	-14.675568	3.956288
-1133.139460	-20.620780	3.966285
-1131.410495	-22.714585	3.976282
-1129.217400	-18.973933	3.986278
-1127.349385	-18.222473	3.996275
-1125.900165	-20.791021	4.006272
-1123.578866	-14.877608	4.016269
-1121.786027	-15.415233	4.026266
-1119.858189	-16.814494	4.036262
-1117.905553	-11.577923	4.046259
-1116.462904	-22.430553	4.056256
-1114.311577	-12.682913	4.066253
-1112.464204	-13.453476	4.076250
-1110.361948	-12.681049	4.086246
-1108.914780	-15.533484	4.096243
-1106.529287	-15.629034	4.106240
-1104.860971	-17.312046	4.116237
-1102.997154	-13.348160	4.126234
-1101.127245	-14.892883	4.136230
-1099.305190	-11.375492	4.146227
-1097.423888	-15.377418	4.156224
-1095.516811	-15.446957	4.166221
-1093.673912	-6.580001	4.176218
-1091.703810	-11.256160	4.186214
-1090.007448	-18.331281	4.196211
-1088.051065	-20.543541	4.206208
-1086.220278	-20.158743	4.216205
-1084.318968	-21.057917	4.226202
-1082.389913	-19.774579	4.236198
-1080.469677	-17.357669	4.246195
-1078.440902	-16.136070	4.256192
-1076.833704	-11.799519	4.266189
-1074.832100	-14.729563	4.276186
-1072.949737	-18.575316	4.286182
-1070.808961	-21.196022	4.296179
-1069.300640	-22.763414	4.306176
-1067.363369	-18.863355	4.316173
-1065.507203	-17.216222	4.326170
-1063.914687	-18.618648	4.336166
-1061.867871	-24.702908	4.346163
-1059.981052	-23.968613	4.356160
-1057.837347	-22.113242	4.366157
-1056.166277	-20.881781	4.376154
-1054.270066	-21.979073	4.386150
-1052.379559	-18.074680	4.396147
-1050.489548	-23.195910	4.406144
-1048.563466	-22.783691	4.416141
-1046.900856	-15.918489	4.426138
-1044.807687	-23.088623	4.436134
-1042.932339	-23.012512	4.446131
-1041.068810	-25.854124	4.456128
-1039.193099	-26.245459	4.466125
-1037.681561	-16.172775	4.476122
-1035.625760	-19.286727	4.486118
-1033.534079	-16.562443	4.496115
-1031.821413	-15.274456	4.506112
-1029.630849	-17.418328	4.516109
-1028.076305	-18.320422	4.526106
-1026.037095	-15.709324	4.536102
-1024.116486	-15.048301	4.546099
-1022.213314	-21.073240	4.556096
-1020.636088	-16.919760	4.566093
-1018.464721	-22.842316	4.576090
-1016.667179	-18.482477	4.586086
-1014.651831	-22.417350	4.596083
-1013.106914	-23.194731	4.606080
-1011.334299	-19.017226	4.616077
-1009.542266	-23.350613	4.626074
-1007.335592	-27.235547	4.636070
-1005.047844	-26.203728	4.646067
-1003.675909	-27.482412	4.656064
-1001.667562	-24.188957	4.666061
-999.874694	-24.674385	4.676058
-997.918307	-22.380035	4.686054
-995.967370	-19.151607	4.696051
-994.029876	-23.752993	4.706048
-992.430684	-19.208250	4.716045
-990.492786	-14.518711	4.726042
-988.569381	-18.527286	4.736038
-986.871016	-16.777482	4.746035
-984.650311	-21.689428	4.756032
-982.951229	-24.634179	4.766029
-981.057933	-18.469007	4.776026
-979.113682	-17.008004	4.786022
-977.443480	-14.156265	4.796019
-975.229417	-17.358635	4.806016
-973.412332	-20.824381	4.816013
-972.038180	-10.219649	4.826010
-969.860596	-16.964254	4.836006
-967.814988	-16.522130	4.846003
-966.069074	-15.168354	4.856000
-964.195815	-18.804137	4.865997
-962.472486	-15.092418	4.875994
-960.794136	-18.122266	4.885990
-958.783925	-15.421203	4.895987
-956.583725	-13.107378	4.905984
-954.663718	-19.807624	4.915981
-953.078626	-20.188738	4.925978
-950.918823	-17.941083	4.935974
-949.211396	-16.893788	4.945971
-947.233304	-25.449196	4.955968
-945.345330	-20.258981	4.965965
-943.479698	-14.345153	4.975962
-941.756698	-24.460903	4.985958
-939.615857	-20.225370	4.995955
-937.909709	-19.473140	5.005952
-936.020652	-19.405451	5.015949
-934.390532	-20.098504	5.025946
-932.580152	-18.687113	5.035942
-930.313472	-14.459058	5.045939
-928.362482	-18.374097	5.055936
-926.740376	-21.524409	5.065933
-924.722079	-24.134876	5.075930
-922.673315	-23.715324	5.085926
-921.200844	-26.112196	5.095923
-919.034285	-24.699319	5.105920
-917.203798	-20.254662	5.115917
-915.368973	-17.430778	5.125914
-913.689895	-13.272977	5.135910
-911.489243	-17.862689	5.145907
-909.748792	-19.377090	5.155904
-908.025428	-19.543427	5.165901
-906.298503	-15.238525	5.175898
-904.348873	-11.637156	5.185894
-901.809158	-20.981834	5.195891
-900.534644	-19.239995	5.205888
-898.365876	-19.425427	5.215885
-896.712095	-19.620106	5.225882
-894.946423	-14.808207	5.235878
-892.884172	-15.682429	5.245875
-890.890015	-20.251742	5.255872
-889.033381	-24.102714	5.265869
-887.206561	-17.151529	5.275866
-885.594892	-13.546643	5.285862
-883.212077	-23.041489	5.295859
-881.545672	-15.033548	5.305856
-879.865587	-15.429799	5.315853
-877.913084	-14.353733	5.325850
-875.931346	-19.426337	5.335846
-874.082120	-21.564449	5.345843
-872.353822	-26.034398	5.355840
-870.302733	-20.519650	5.365837
-868.502534	-22.002518	5.375834
-866.620451	-18.451901	5.385830
-864.799142	-16.195844	5.395827
-862.754602	-20.245793	5.405824
-860.604286	-22.253596	5.415821
-859.239400	-20.385648	5.425818
-857.193727	-16.186930	5.435814
-855.351105	-20.209331	5.445811
-853.763456	-21.411882	5.455808
-851.640549	-17.318668	5.465805
-849.640708	-13.567375	5.475802
-847.737553	-15.717246	5.485798
-846.335435	-18.423371	5.495795
-843.837074	-16.272369	5.505792
-842.312291	-19.132317	5.515789
-840.478826	-16.341314	5.525786
-838.248667	-15.827520	5.535782
-836.453443	-16.482158	5.545779
-834.713770	-21.452874	5.555776
-832.710390	-20.214368	5.565773
-831.026488	-21.755990	5.575770
-829.037417	-24.571717	5.585766
-827.620797	-20.668757	5.595763
-825.500651	-22.816977	5.605760
-823.188585	-26.748594	5.615757
-821.722380	-19.185473	5.625754
-819.631838	-13.222220	5.635750
-817.670987	-13.595408	5.645747
-815.995566	-19.209560	5.655744
-814.201062	-18.311880	5.665741
-812.103233	-15.828387	5.675738
-810.164616	-15.545876	5.685734
-808.537404	-20.525442	5.695731
-806.668322	-18.104861	5.705728
-804.516502	-18.538563	5.715725
-803.061488	-19.528818	5.725722
-800.973752	-19.930167	5.735718
-798.945105	-15.608668	5.745715
-797.304488	-16.091715	5.755712
-795.290803	-16.072255	5.765709
-793.437116	-13.406031	5.775706
-791.611768	-15.728168	5.785702
-789.683152	-15.823008	5.795699
-787.795820	-13.588495	5.805696
-785.830012	-10.911762	5.815693
-784.085119	-12.936810	5.825690
-782.117274	-12.033651	5.835686
-780.280875	-9.952051	5.845683
-778.367820	-10.816541	5.855680
-776.439050	-14.538427	5.865677
-774.618896	-9.864617	5.875674
-773.037208	-6.703301	5.885670
-770.887659	-11.472628	5.895667
-769.163177	-11.793787	5.905664
-767.160021	-13.618507	5.915661
-765.256018	-15.241052	5.925658
-763.344293	-14.988943	5.935654
-761.271069	-13.358884	5.945651
-759.686413	-11.991812	5.955648
-757.632233	-7.252752	5.965645
-756.238477	-11.827063	5.975642
-754.110860	-17.396596	5.985638
-752.088844	-21.614968	5.995635
-750.216313	-23.200891	6.005632
-748.721283	-16.243934	6.015629
-746.516391	-21.835282	6.025626
-744.677256	-14.532240	6.035622
-742.733740	-16.473730	6.045619
-740.821727	-17.393289	6.055616
-738.957537	-12.251200	6.065613
-736.892281	-18.881335	6.075610
-735.347170	-13.751413	6.085606
-733.471787	-15.606215	6.095603
-731.635124	-16.586360	6.105600
-729.451590	-15.223388	6.115597
-727.850713	-20.625033	6.125594
-725.907287	-12.209633	6.135590
-723.975762	-12.789647	6.145587
-722.283480	-15.073099	6.155584
-720.372145	-18.207913	6.165581
-718.289813	-15.815021	6.175578
-716.621054	-19.264772	6.185574
-714.649984	-20.485867	6.195571
-712.624884	-17.384314	6.205568
-710.813243	-19.391552	6.215565
-708.872861	-18.288143	6.225562
-707.383085	-18.655441	6.235558
-705.280654	-18.099004	6.245555
-703.043235	-12.798618	6.255552
-701.463242	-20.533876	6.265549
-699.541251	-17.202666	6.275546
-697.772036	-14.961837	6.285542
-696.004477	-15.100343	6.295539
-694.142455	-10.633694	6.305536
-692.225601	-11.664520	6.315533
-690.174146	-15.969658	6.325530
-688.126252	-13.601237	6.335526
-686.414846	-15.854560	6.345523
-684.631084	-14.462406	6.355520
-682.697918	-21.537205	6.365517
-680.859717	-13.927626	6.375514
-678.906527	-18.021253	6.385510
-677.161942	-18.664521	6.395507
-675.331988	-18.138735	6.405504
-673.282401	-15.522663	6.415501
-671.454321	-20.692141	6.425498
-669.601672	-15.039702	6.435494
-667.970428	-12.419944	6.445491
-665.624631	-14.022996	6.455488
-663.908974	-18.582369	6.465485
-662.049907	-17.568566	6.475482
-660.412045	-12.522888	6.485478
-658.159898	-9.915480	6.495475
-656.480834	-10.592478	6.505472
-654.578791	-20.364009	6.515469
-652.789460	-10.752279	6.525466
-650.739608	-14.164975	6.535462
-648.605241	-13.840970	6.545459
-647.409360	-12.354861	6.555456
-645.045598	-17.232519	6.565453
-643.364795	-15.365964	6.575450
-641.511948	-11.876806	6.585446
-639.833548	-16.152302	6.595443
-637.691485	-8.752292	6.605440
-635.852371	-17.582128	6.615437
-634.081946	-15.879893	6.625434
-631.941864	-15.188872	6.635430
-630.096997	-17.837709	6.645427
-628.446971	-19.537998	6.655424
-626.498780	-22.274395	6.665421
-624.521433	-14.958592	6.675418
-622.494601	-12.383052	6.685414
-620.637669	-17.102343	6.695411
-618.977259	-17.117878	6.705408
-617.128194	-19.694740	6.715405
-615.235911	-11.361073	6.725402
-613.292988	-19.367431	6.735398
-611.667191	-18.523174	6.745395
-609.662106	-20.878627	6.755392
-607.616326	-22.034197	6.765389
-605.934205	-20.212040	6.775386
-603.821737	-18.866020	6.785382
-602.070540	-20.636141	6.795379
-600.125536	-19.187572	6.805376
-598.059287	-17.878377	6.815373
-596.434739	-17.322873	6.825370
-594.727973	-16.905247	6.835366
-592.786094	-15.484594	6.845363
-590.816295	-15.675856	6.855360
-588.968844	-16.444447	6.865357
-587.110316	-10.552863	6.875354
-585.310362	-10.723305	6.885350
-583.134807	-15.772956	6.895347
-581.436076	-21.400154	6.905344
-579.473918	-15.918299	6.915341
-577.491703	-19.839631	6.925338
-575.643374	-15.497021	6.935334
-574.148438	-14.016011	6.945331
-572.158117	-17.779152	6.955328
-569.871745	-15.470826	6.965325
-568.149645	-21.753890	6.975322
-566.444887	-23.901850	6.985318
-564.355590	-18.525560	6.995315
-562.650292	-25.115424	7.005312
-561.052029	-21.036034	7.015309
-558.823895	-17.674654	7.025306
-556.780434	-14.127449	7.035302
-555.147945	-12.515233	7.045299
-553.333395	-13.196431	7.055296
-551.379437	-18.068545	7.065293
-549.619463	-12.374358	7.075290
-547.942348	-8.010690	7.085286
-545.616016	-10.167916	7.095283
-544.009409	-9.794258	7.105280
-541.879929	-19.174121	7.115277
-540.038131	-21.433958	7.125274
-538.035697	-21.827768	7.135270
-536.639417	-13.166900	7.145267
-534.602418	-22.724625	7.155264
-532.763502	-21.696448	7.165261
-530.692992	-20.323134	7.175258
-528.869749	-17.648675	7.185254
-526.834392	-8.518261	7.195251
-524.934571	-10.878939	7.205248
-523.571968	-10.136276	7.215245
-521.593544	-13.210598	7.225242
-519.462648	-6.939276	7.235238
-517.666071	-12.924713	7.245235
-515.820612	-7.899450	7.255232
-513.657380	-14.739279	7.265229
-511.868372	-15.301097	7.275226
-510.106565	-16.517026	7.285222
-508.343404	-18.517951	7.295219
-506.333888	-14.126812	7.305216
-504.590718	-11.646398	7.315213
-502.539413	-17.486181	7.325210
-500.732538	-15.309639	7.335206
-498.937821	-16.862414	7.345203
-496.761872	-17.902884	7.355200
-495.163843	-15.962999	7.365197
-493.276795	-19.240610	7.375194
-491.303891	-15.734186	7.385190
-489.336386	-20.028910	7.395187
-487.703150	-17.058796	7.405184
-485.587318	-14.258916	7.415181
-483.975183	-19.927487	7.425178
-482.015140	-17.683809	7.435174
-480.131113	-17.333885	7.445171
-478.331184	-10.337000	7.455168
-476.375730	-12.108071	7.465165
-474.473006	-14.075993	7.475162
-472.247602	-17.936601	7.485158
-470.668857	-18.387437	7.495155
-468.911321	-14.772386	7.505152
-467.001277	-16.574093	7.515149
-465.242485	-11.089661	7.525146
-463.135739	-13.707559	7.535142
-461.440405	-13.098526	7.545139
-459.346219	-16.322344	7.555136
-457.220985	-15.987234	7.565133
-455.701231	-20.496235	7.575130
-453.759468	-19.516001	7.585126
-452.301446	-11.812354	7.595123
-450.122558	-16.150279	7.605120
-447.923191	-16.937061	7.615117
-446.451111	-15.638646	7.625114
-444.341037	-12.984658	7.635110
-442.586414	-11.827679	7.645107
-440.644843	-10.266317	7.655104
-438.807848	-20.390490	7.665101
-436.906694	-16.702027	7.675098
-434.901047	-15.910408	7.685094
-432.978130	-16.747775	7.695091
-431.398400	-16.751876	7.705088
-429.350225	-23.543257	7.715085
-427.453705	-18.794513	7.725082
-425.830935	-12.381964	7.735078
-424.285724	-12.990056	7.745075
-421.996549	-12.305281	7.755072
-419.897839	-15.278722	7.765069
-418.233110	-16.799628	7.775066
-416.047386	-17.085228	7.785062
-414.401618	-20.640060	7.795059
-412.586980	-16.078767	7.805056
-410.888685	-21.449981	7.815053
-408.661362	-16.742987	7.825050
-406.908185	-22.550880	7.835046
-404.877595	-18.164596	7.845043
-403.164330	-16.465692	7.855040
-401.340153	-19.958997	7.865037
-399.421449	-23.547924	7.875034
-397.816716	-21.361135	7.885030
-395.580185	-19.172583	7.895027
-393.767023	-15.687941	7.905024
-391.905874	-17.025442	7.915021
-390.130001	-16.179730	7.925018
-387.934621	-20.529707	7.935014
-386.230394	-14.676480	7.945011
-384.567886	-12.197309	7.955008
-382.759826	-15.558547	7.965005
-380.519664	-19.723025	7.975002
-378.567221	-22.163048	7.984998
-376.926543	-14.839060	7.994995
-375.018764	-13.682798	8.004992
-373.041596	-17.683695	8.014989
-371.351844	-21.687652	8.024986
-369.511847	-21.349559	8.034982
-367.642215	-17.755485	8.044979
-365.387757	-18.519407	8.054976
-363.768830	-13.776819	8.064973
-361.738474	-19.145750	8.074970
-359.967295	-14.282195	8.084966
-358.369695	-15.375478	8.094963
-356.177417	-15.471006	8.104960
-354.303383	-15.795214	8.114957
-352.532552	-18.893104	8.124954
-350.576622	-16.125997	8.134950
-348.706174	-15.833804	8.144947
-346.670985	-15.839504	8.154944
-345.021212	-17.999062	8.164941
-343.262927	-17.944763	8.174938
-341.114416	-20.458691	8.184934
-339.543608	-11.470267	8.194931
-337.570564	-12.130813	8.204928
-335.656091	-14.094188	8.214925
-333.618311	-16.490954	8.224922
-331.626488	-20.789438	8.234918
-330.103432	-17.034210	8.244915
-328.119970	-12.288207	8.254912
-326.206692	-11.001723	8.264909
-324.563689	-23.504464	8.274906
-322.413217	-17.427146	8.284902
-320.406706	-14.105949	8.294899
-318.661575	-18.316093	8.304896
-316.926987	-13.925111	8.314893
-315.105835	-20.928073	8.324890
-313.154712	-22.391989	8.334886
-311.364293	-19.783176	8.344883
-309.378616	-26.613436	8.354880
-307.303136	-22.572145	8.364877
-305.723951	-19.501690	8.374874
-303.645496	-14.946103	8.384870
-301.741856	-18.278327	8.394867
-300.316133	-15.900254	8.404864
-298.108275	-17.174599	8.414861
-295.931729	-17.861279	8.424858
-294.133215	-19.761899	8.434854
-292.493086	-21.144575	8.444851
-290.639148	-15.596241	8.454848
-288.926368	-19.586451	8.464845
-286.911739	-24.101709	8.474842
-285.003524	-20.426880	8.484838
-283.293119	-23.178740	8.494835
-280.758523	-20.300245	8.504832
-279.227743	-17.492060	8.514829
-277.647621	-22.748003	8.524826
-275.721216	-11.863019	8.534822
-273.306723	-16.934754	8.544819
-271.961974	-16.114882	8.554816
-270.027593	-20.895230	8.564813
-267.931150	-20.528513	8.574810
-266.341452	-21.571524	8.584807
-264.184819	-19.706430	8.594803
-262.753921	-18.390273	8.604800
-260.584813	-21.756942	8.614797
-258.756947	-18.020316	8.624794
-256.723594	-21.818498	8.634791
-254.762543	-28.395297	8.644787
-252.909997	-24.885251	8.654784
-251.155189	-21.438555	8.664781
-249.644489	-21.036759	8.674778
-247.419317	-23.818646	8.684775
-245.549786	-16.253173	8.694771
-243.475426	-16.427679	8.704768
-241.730120	-20.625165	8.714765
-239.778704	-25.856655	8.724762
-237.864932	-23.409587	8.734759
-236.114420	-23.035003	8.744755
-234.047567	-22.731433	8.754752
-232.492105	-18.226531	8.764749
-230.542477	-23.015598	8.774746
-228.565723	-21.930231	8.784743
-226.695872	-20.625684	8.794739
-225.156552	-19.942634	8.804736
-223.067710	-19.350441	8.814733
-221.186906	-20.938858	8.824730
-219.315713	-21.511997	8.834727
-217.375849	-26.042112	8.844723
-215.486163	-22.440062	8.854720
-213.659959	-28.842144	8.864717
-211.612609	-30.581876	8.874714
-209.922850	-24.108805	8.884711
-208.007401	-26.029602	8.894707
-206.346240	-29.275684	8.904704
-204.301373	-28.319595	8.914701
-202.497980	-29.579836	8.924698
-200.501368	-33.250521	8.934695
-198.752283	-28.741760	8.944691
-196.772230	-29.474367	8.954688
-194.771483	-23.221448	8.964685
-193.004709	-29.340858	8.974682
-191.113332	-27.780756	8.984679
-189.294770	-23.341497	8.994675
-187.449131	-24.060542	9.004672
-185.244701	-29.687649	9.014669
-183.789313	-28.375354	9.024666
-181.653720	-27.220553	9.034663
-179.811999	-25.551460	9.044659
-178.142922	-22.967394	9.054656
-176.402708	-28.053022	9.064653
-174.338979	-29.040556	9.074650
-172.285627	-27.847358	9.084647
-170.425610	-21.579855	9.094643
-168.774010	-21.994749	9.104640
-166.787779	-22.772531	9.114637
-164.806943	-25.216916	9.124634
-162.856807	-24.351471	9.134631
-161.271025	-22.523095	9.144627
-159.201484	-22.079354	9.154624
-157.279021	-28.593079	9.164621
-155.414345	-29.070387	9.174618
-153.835963	-25.783371	9.184615
-151.824686	-27.102011	9.194611
-149.898123	-26.074890	9.204608
-147.936611	-24.818067	9.214605
-146.058178	-26.169192	9.224602
-144.317450	-19.050478	9.234599
-142.485869	-23.490623	9.244595
-140.518202	-21.508417	9.254592
-138.304046	-23.408923	9.264589
-136.966845	-21.468231	9.274586
-134.867622	-19.702812	9.284583
-132.844043	-16.984212	9.294579
-131.140976	-16.815152	9.304576
-129.172418	-19.641258	9.314573
-127.191516	-22.584602	9.324570
-125.606349	-22.898861	9.334567
-123.662937	-15.930896	9.344563
-121.700053	-21.119916	9.354560
-120.037036	-21.860301	9.364557
-117.880086	-24.340644	9.374554
-116.166932	-23.099435	9.384551
-114.315358	-26.352154	9.394547
-112.463613	-14.990872	9.404544
-110.306972	-15.584206	9.414541
-108.426544	-15.457638	9.424538
-106.740147	-14.289526	9.434535
-104.858536	-12.170393	9.444531
-102.983708	-14.570974	9.454528
-101.009673	-17.655316	9.464525
-99.175844	-15.961214	9.474522
-97.486613	-21.384468	9.484519
-95.521914	-16.384201	9.494515
-93.950996	-14.327604	9.504512
-91.740896	-17.580661	9.514509
-89.741768	-17.637237	9.524506
-87.794535	-18.149770	9.534503
-85.976470	-17.026335	9.544499
-84.283265	-17.094104	9.554496
-82.160672	-12.403242	9.564493
-80.566835	-16.398024	9.574490
-78.519774	-11.549837	9.584487
-76.840844	-15.813997	9.594483
-75.050804	-16.519351	9.604480
-72.906583	-15.939020	9.614477
-70.928974	-21.302466	9.624474
-69.111742	-28.467275	9.634471
-67.203399	-21.541039	9.644467
-65.553899	-13.153946	9.654464
-63.811288	-22.151172	9.664461
-61.719914	-19.136992	9.674458
-59.792199	-20.382223	9.684455
-57.761580	-17.971016	9.694451
-56.218068	-20.719785	9.704448
-54.067025	-20.129473	9.714445
-51.999499	-19.093179	9.724442
-50.621616	-19.371165	9.734439
-48.687626	-22.464868	9.744435
-46.644230	-16.899183	9.754432
-44.929373	-20.581649	9.764429
-42.773060	-22.757071	9.774426
-41.172033	-23.959648	9.784423
-39.422483	-23.207377	9.794419
-37.368387	-16.326470	9.804416
-35.347498	-19.689830	9.814413
-33.498897	-23.567316	9.824410
-31.383163	-20.883858	9.834407
-30.014769	-20.692922	9.844403
-27.969739	-22.741626	9.854400
-26.056440	-17.497823	9.864397
-24.033734	-18.412369	9.874394
-22.200608	-19.020339	9.884391
-20.314290	-28.438376	9.894387
-18.581601	-17.195399	9.904384
-16.739185	-17.541148	9.914381
-14.679770	-23.144982	9.924378
-13.077678	-21.747028	9.934375
-11.020411	-20.920653	9.944371
-9.051090	-14.217261	9.954368
-7.293466	-10.843461	9.964365
-6.213778	-3.376017	9.974362
-4.522248	23.491911	9.984359
-2.944398	63.657847	9.994355
-1.416074	120.126090	10.004352
0.000000	168.571183	10.009357
0.588206	192.858611	10.014362
1.584001	211.843688	10.019367
2.122115	244.078060	10.024371
2.551835	253.352103	10.029376
2.457424	259.778008	10.034381
2.412050	262.338618	10.039386
2.944228	261.561529	10.044391
2.473078	275.354026	10.049395
3.076770	278.047670	10.054400
3.049884	286.574495	10.059405
3.336286	290.585126	10.064410
3.391156	290.155422	10.069415
3.294844	288.958148	10.074419
2.974401	281.374847	10.079424
3.246898	278.650509	10.084429
3.305746	291.962645	10.089434
3.495476	289.226273	10.094439
3.269466	303.520627	10.099443
3.326121	304.710277	10.104448
3.588838	305.684121	10.109453
3.681268	299.624633	10.114458
3.914713	299.850889	10.119463
3.679657	300.664414	10.124467
3.686278	285.608885	10.129472
3.599167	288.387482	10.134477
3.375476	297.313157	10.139482
3.875941	304.434305	10.144487
3.633792	314.142002	10.149491
3.963336	315.187195	10.154496
3.883144	316.132149	10.159501
4.226341	323.677387	10.164506
4.227915	319.974318	10.169511
3.791279	328.421433	10.174515
4.005930	316.964663	10.179520
4.107185	323.482398	10.184525
4.177068	327.489725	10.189530
4.125846	316.048553	10.194535
4.229313	322.304143	10.199539
4.217904	325.297769	10.204544
4.165248	325.916612	10.209549
4.450507	331.043997	10.214554
4.168893	331.967459	10.219559
4.285375	330.241044	10.224563
4.386708	331.081347	10.229568
4.139170	332.888837	10.234573
4.028129	344.122741	10.239578
4.900048	361.782540	10.244583
5.002264	371.170402	10.249587
4.869510	365.257198	10.254592
4.857834	359.387767	10.259597
4.912391	371.170907	10.264602
5.018131	355.449744	10.269607
4.575509	360.604921	10.274611
4.981473	371.903051	10.279616
5.401981	375.996403	10.284621
4.900538	372.037637	10.289626
5.118893	368.563349	10.294631
5.306664	381.774574	10.299635
5.432836	367.221901	10.304640
4.936891	366.053666	10.309645
5.371042	371.717176	10.314650
5.414974	367.471137	10.319655
5.383655	380.244185	10.324659
5.722237	371.308262	10.329664
5.393757	360.447480	10.334669
5.019114	367.634117	10.339674
5.459456	370.713405	10.344679
5.499131	378.478983	10.349683
5.463240	382.113661	10.354688
5.550203	389.900090	10.359693
5.366192	392.451294	10.364698
5.736760	385.715003	10.369703
5.716584	387.782724	10.374707
5.808116	388.026886	10.379712
6.001217	393.780895	10.384717
5.747710	399.686571	10.389722
5.803902	400.961464	10.394727
5.959291	400.835869	10.399731
5.600197	394.345274	10.404736
6.201909	405.621671	10.409741
6.204840	416.544116	10.414746
6.135530	399.764224	10.419751
6.134856	418.001696	10.424755
6.152122	414.001188	10.429760
6.595068	421.789207	10.434765
6.089465	437.101339	10.439770
6.559655	427.089329	10.444775
6.518419	423.377291	10.449779
6.568182	429.450666	10.454784
6.778322	431.631481	10.459789
6.414904	429.219871	10.464794
6.710110	432.257662	10.469799
6.639474	432.931420	10.474803
6.834964	435.685473	10.479808
7.006634	436.842595	10.484813
6.641987	439.998250	10.489818
6.910702	431.276877	10.494823
6.846605	437.488274	10.499827
6.619984	442.814047	10.504832
6.834926	444.516244	10.509837
6.684063	445.032475	10.514842
7.083811	433.013041	10.519847
6.912153	441.558316	10.524851
6.807566	445.481531	10.529856
6.775987	445.672785	10.534861
6.973167	446.483614	10.539866
7.283250	456.022894	10.544871
7.506522	469.818363	10.549875
7.757504	460.782808	10.554880
7.401752	450.457783	10.559885
7.395908	446.254355	10.564890
7.821453	451.994969	10.569895
7.643402	449.217873	10.574899
7.555648	452.349869	10.579904
7.614282	446.836647	10.584909
7.259150	463.993641	10.589914
7.762972	459.869780	10.594919
7.948699	478.654807	10.599923
7.791827	480.859471	10.604928
7.737209	481.358775	10.609933
7.584105	477.853816	10.614938
8.319997	474.282763	10.619943
8.063878	479.815120	10.624947
8.163697	478.009337	10.629952
8.320132	482.480757	10.634957
7.810969	488.349969	10.639962
8.012412	477.762574	10.644967
7.960072	485.312632	10.649971
8.355710	485.087210	10.654976
8.491093	479.443454	10.659981
8.092163	482.019490	10.664986
8.323185	477.896554	10.669991
8.314532	486.600374	10.674995
8.446101	484.262782	10.680000
8.496692	480.433573	10.685005
8.390044	489.949450	10.690010
8.521184	481.466050	10.695015
8.746425	489.192627	10.700019
8.655613	483.980794	10.705024
8.378298	488.880972	10.710029
8.326209	496.050920	10.715034
9.092880	502.076217	10.720039
8.930882	510.809242	10.725043
9.135803	501.749467	10.730048
9.075231	504.473405	10.735053
8.783877	494.190121	10.740058
8.903292	499.146883	10.745063
8.915968	509.515866	10.750067
9.340046	515.013869	10.755072
9.442010	521.698750	10.760077
9.218226	520.248953	10.765082
9.606195	507.551614	10.770087
9.165023	509.252804	10.775091
8.932342	500.275443	10.780096
9.333307	508.048126	10.785101
9.192349	520.119636	10.790106
9.595139	520.801473	10.795111
9.517829	521.700245	10.800115
9.434233	512.352140	10.805120
9.567952	520.351974	10.810125
9.516771	526.144998	10.815130
9.748746	513.784797	10.820135
9.751043	510.223502	10.825139
9.819102	515.762519	10.830144
9.658188	520.998986	10.835149
9.840192	525.038951	10.840154
9.868993	517.772013	10.845159
9.797741	527.408436	10.850163
9.848654	524.944918	10.855168
10.173977	528.703384	10.860173
9.799001	533.284813	10.865178
9.779669	524.803308	10.870183
9.828842	544.130638	10.875187
10.328563	544.382242	10.880192
10.676542	545.325157	10.885197
10.518217	552.196660	10.890202
10.596349	534.443689	10.895207
10.196436	542.825140	10.900211
10.578281	539.411476	10.905216
10.301782	535.654924	10.910221
10.211521	549.995682	10.915226
10.906008	554.192057	10.920231
10.940215	556.653285	10.925235
10.982234	544.804367	10.930240
10.767751	532.346611	10.935245
10.769456	534.623770	10.940250
10.884473	531.419837	10.945255
10.605752	533.500429	10.950259
10.782373	540.755355	10.955264
11.038242	545.949011	10.960269
10.872666	560.101502	10.965274
10.926953	556.850475	10.970279
11.041848	559.391882	10.975283
10.997274	559.500047	10.980288
11.301269	562.211584	10.985293
11.043306	555.700054	10.990298
11.443039	552.991646	10.995303
11.243467	553.157650	11.000307
11.296760	559.446578	11.005312
11.589136	555.667102	11.010317
11.254623	558.868442	11.015322
11.441388	558.786731	11.020327
11.297283	554.616364	11.025331
11.401627	562.023190	11.030336
11.596718	559.213368	11.035341
11.547296	561.105991	11.040346
11.329488	554.302604	11.045351
11.104830	568.382518	11.050355
11.458605	564.870814	11.055360
11.779944	575.288393	11.060365
11.880825	595.356660	11.065370
12.192914	585.189971	11.070375
12.127601	583.973534	11.075379
12.052906	570.403681	11.080384
11.889916	563.952700	11.085389
12.064981	580.982685	11.090394
12.154355	572.764536	11.095399
12.009676	586.762319	11.100403
11.892044	587.583941	11.105408
11.915172	585.205276	11.110413
12.022659	592.794559	11.115418
12.303158	588.477605	11.120423
12.254293	596.938724	11.125427
12.536028	591.367784	11.130432
12.659328	590.444567	11.135437
12.556342	596.260076	11.140442
12.636793	590.440519	11.145447
12.601502	595.636474	11.150451
12.685804	593.867847	11.155456
12.652643	593.363858	11.160461
12.477531	600.954060	11.165466
12.737368	599.523321	11.170471
12.694869	600.810818	11.175475
12.450476	594.123627	11.180480
12.515714	600.850676	11.185485
12.973476	616.498240	11.190490
13.145344	620.456263	11.195495
13.042816	629.284750	11.200499
13.159667	625.157115	11.205504
13.377695	621.581098	11.210509
12.966930	624.767803	11.215514
13.325956	619.486539	11.220519
12.827682	624.275335	11.225523
12.759875	626.218211	11.230528
13.368437	630.253256	11.235533
13.137144	640.170768	11.240538
13.484624	623.961287	11.245543
13.295031	631.864502	11.250547
13.346057	631.703507	11.255552
13.444985	628.783630	11.260557
13.437295	627.994854	11.265562
13.610896	625.621359	11.270567
13.517806	631.887930	11.275571
13.489307	635.442637	11.280576
13.484339	643.505663	11.285581
13.904140	653.033882	11.290586
14.295402	642.781979	11.295591
14.487282	648.551267	11.300595
13.798396	631.351851	11.305600
14.244471	631.965285	11.310605
14.168713	624.947591	11.315610
14.117754	618.045016	11.320615
13.996160	625.485546	11.325619
13.850545	619.273064	11.330624
13.912422	627.386137	11.335629
14.306983	645.500926	11.340634
14.722471	643.650295	11.345639
14.494390	655.493728	11.350643
14.456427	638.168405	11.355648
14.525357	622.619208	11.360653
14.495324	629.115439	11.365658
14.406999	621.984623	11.370663
14.717826	637.217214	11.375667
14.908498	639.874295	11.380672
14.708551	624.536730	11.385677
14.291184	630.306981	11.390682
14.727088	640.773361	11.395687
14.412925	647.728905	11.400691
14.529063	647.773587	11.405696
14.712630	648.838147	11.410701
14.799834	650.089191	11.415706
14.969146	647.419882	11.420711
14.887201	660.897540	11.425715
15.196949	648.726689	11.430720
15.315049	649.506774	11.435725
15.163889	649.223471	11.440730
15.512815	654.309275	11.445735
15.515705	652.320217	11.450739
15.250943	656.097132	11.455744
15.356468	656.776711	11.460749
15.498044	653.498335	11.465754
15.336495	659.686731	11.470759
15.313526	665.365703	11.475763
15.289909	657.815292	11.480768
15.603305	658.655700	11.485773
15.269106	655.804899	11.490778
15.309230	655.480047	11.495783
15.187230	654.883771	11.500787
15.278908	668.510378	11.505792
15.778740	675.420482	11.510797
15.593223	687.030049	11.515802
15.918034	682.315667	11.520807
15.609083	688.785441	11.525811
15.625690	683.931752	11.530816
16.053911	688.743912	11.535821
15.729178	686.997144	11.540826
15.710042	681.924420	11.545831
15.768647	683.874741	11.550835
15.806033	698.203171	11.555840
16.208628	695.502955	11.560845
16.445239	706.412792	11.565850
16.617472	703.645228	11.570855
16.629806	694.143708	11.575859
16.424462	683.889152	11.580864
16.707808	679.598528	11.585869
16.675259	682.491511	11.590874
16.920491	676.013220	11.595879
16.779833	681.440497	11.600883
16.508946	681.518520	11.605888
16.910869	677.988071	11.610893
16.682444	690.963945	11.615898
16.765311	686.430090	11.620903
16.463100	694.425425	11.625907
16.731230	689.709041	11.630912
16.990971	680.403058	11.635917
16.624657	687.896845	11.640922
16.385802	687.019555	11.645927
16.741984	688.531294	11.650931
16.597709	694.496944	11.655936
16.984700	708.645822	11.660941
16.993310	710.347841	11.665946
17.418995	707.888391	11.670951
17.301158	711.484965	11.675955
17.395013	712.547279	11.680960
17.325565	711.412711	11.685965
17.034014	720.555280	11.690970
17.352232	709.151866	11.695975
17.575242	717.191977	11.700979
17.672675	714.687100	11.705984
17.588500	710.533151	11.710989
17.256239	720.803533	11.715994
17.992827	710.696009	11.720999
17.522132	727.428578	11.726003
17.714897	721.359220	11.731008
17.916753	707.076438	11.736013
17.812005	713.703695	11.741018
18.002306	713.839848	11.746023
17.931482	719.732286	11.751027
17.938334	709.885456	11.756032
18.176498	719.682411	11.761037
17.761270	714.161868	11.766042
18.153907	709.876672	11.771047
17.863608	719.589951	11.776051
17.902997	719.144567	11.781056
17.985032	716.489955	11.786061
17.649763	715.251902	11.791066
17.947855	712.718964	11.796071
17.704315	717.082347	11.801075
18.251534	728.209191	11.806080
18.358328	727.585883	11.811085
18.441982	738.545375	11.816090
18.475196	738.187715	11.821095
18.444658	746.065624	11.826099
18.484773	750.080970	11.831104
18.660316	736.742313	11.836109
18.678012	733.327543	11.841114
18.779454	735.253691	11.846119
18.630534	742.074103	11.851123
18.665822	741.662492	11.856128
18.752333	741.495836	11.861133
18.327714	743.405742	11.866138
18.672639	739.119473	11.871143
18.924387	735.750171	11.876147
18.644581	743.156852	11.881152
18.913438	751.557136	11.886157
18.800696	753.611285	11.891162
18.912822	757.268185	11.896167
19.099343	758.191919	11.901171
19.602447	763.255538	11.906176
19.718542	763.371986	11.911181
19.240016	759.829754	11.916186
19.675641	739.231976	11.921191
19.489457	733.924866	11.926195
19.166304	739.037462	11.931200
19.243307	738.448869	11.936205
19.256778	760.590219	11.941210
19.492494	753.708884	11.946215
19.238466	760.364702	11.951219
19.439159	757.117090	11.956224
19.880104	753.792521	11.961229
19.343602	767.652678	11.966234
19.778771	764.428385	11.971239
19.711453	765.625230	11.976243
19.394264	758.612859	11.981248
19.713074	763.004059	11.986253
19.947231	769.608041	11.991258
19.882360	783.780960	11.996263
19.812391	788.376904	12.001267
20.065659	783.326148	12.006272
20.169558	782.148944	12.011277
19.898877	792.408766	12.016282
20.303467	786.087955	12.021287
20.471158	786.502134	12.026291
20.587227	785.423924	12.031296
20.487714	774.229025	12.036301
20.217048	768.399159	12.041306
20.503948	755.645968	12.046311
20.350020	763.254166	12.051315
20.365202	759.941515	12.056320
20.596020	749.361067	12.061325
20.553916	767.965955	12.066330
20.855405	762.149714	12.071335
20.205159	745.671832	12.076339
20.320964	737.577909	12.081344
20.324027	734.707998	12.086349
19.943536	732.774555	12.091354
20.152076	728.760801	12.096359
20.061269	730.945503	12.101363
20.072127	726.768506	12.106368
20.318407	727.980780	12.111373
19.669645	737.682640	12.116378
20.205363	727.937546	12.121383
20.085734	727.448920	12.126387
19.875058	730.826106	12.131392
20.351723	732.701082	12.136397
19.697217	741.836891	12.141402
20.271770	735.039519	12.146407
20.169294	739.457688	12.151411
20.077164	730.051661	12.156416
20.324643	738.098133	12.161421
20.057473	736.241242	12.166426
20.378322	741.871715	12.171431
19.952807	743.276302	12.176435
19.845019	737.823421	12.181440
19.932587	734.202734	12.186445
19.916566	759.011729	12.191450
20.244382	761.500288	12.196455
20.154410	765.507999	12.201459
20.247362	764.852989	12.206464
20.312395	750.886906	12.211469
19.882371	741.824164	12.216474
20.539086	747.714127	12.221479
20.195076	745.498081	12.226483
20.210085	738.739484	12.231488
20.321862	737.367043	12.236493
19.912811	739.778351	12.241498
20.440971	740.249376	12.246503
20.116267	742.148866	12.251507
19.896370	745.905243	12.256512
20.077108	733.346428	12.261517
20.250593	741.047488	12.266522
20.062566	735.443386	12.271527
20.128537	741.064044	12.276531
20.212442	738.669352	12.281536
20.498767	742.233015	12.286541
20.037700	748.071788	12.291546
19.983928	741.721590	12.296551
20.061435	750.872342	12.301555
20.196372	749.010457	12.306560
20.697726	749.317007	12.311565
20.228325	743.684444	12.316570
20.254482	745.369475	12.321575
20.630601	750.055913	12.326579
20.461610	748.356843	12.331584
20.764153	737.235056	12.336589
20.333210	731.415785	12.341594
19.985119	716.229497	12.346599
19.984904	717.708187	12.351603
20.153074	716.161158	12.356608
20.293347	706.831632	12.361613
20.062334	707.657150	12.366618
20.253602	710.039733	12.371623
20.154772	718.200569	12.376627
20.084448	714.684713	12.381632
20.409391	710.404006	12.386637
20.186612	719.143694	12.391642
20.433539	711.342716	12.396647
20.303341	717.599471	12.401651
20.202338	714.840788	12.406656
20.466753	713.291814	12.411661
20.224138	724.281254	12.416666
20.153463	715.734491	12.421671
20.144400	718.261790	12.426675
20.267853	715.881297	12.431680
20.210744	718.909892	12.436685
19.928283	725.393593	12.441690
20.063103	717.528483	12.446695
19.780619	712.924357	12.451699
19.869317	720.567960	12.456704
19.891822	713.574767	12.461709
20.008535	722.022168	12.466714
19.952075	720.362718	12.471719
20.030496	717.624307	12.476723
20.450631	713.702189	12.481728
20.417701	714.699561	12.486733
20.125473	716.824125	12.491738
20.280320	716.927295	12.496743
20.240390	722.969363	12.501747
20.118079	726.544575	12.506752
20.500567	719.108362	12.511757
20.044214	721.513018	12.516762
20.053537	722.134608	12.521767
19.929399	720.445736	12.526771
19.981572	725.965288	12.531776
20.380927	726.957587	12.536781
20.204129	730.289942	12.541786
20.340853	722.630337	12.546791
20.317392	729.054595	12.551795
20.203375	726.858645	12.556800
20.203113	709.254384	12.561805
20.043517	712.475960	12.566810
20.064361	698.730673	12.571815
20.136745	713.172607	12.576819
20.138632	718.881544	12.581824
20.243437	703.355715	12.586829
20.106343	705.849811	12.591834
20.153738	695.746553	12.596839
20.090189	704.209289	12.601843
19.950411	704.590495	12.606848
20.037423	710.461698	12.611853
20.205347	714.230336	12.616858
20.437243	713.756614	12.621863
20.150451	711.971460	12.626867
20.083603	713.691823	12.631872
20.149896	700.907626	12.636877
19.737554	714.485343	12.641882
19.906550	714.774720	12.646887
20.089227	725.231083	12.651891
20.412057	732.803442	12.656896
20.561073	720.731503	12.661901
19.983038	707.922320	12.666906
20.254579	701.754455	12.671911
20.314290	703.885969	12.676915
20.003093	702.004563	12.681920
20.258702	697.730974	12.686925
20.045413	706.304334	12.691930
20.126999	700.006690	12.696935
20.145039	703.486176	12.701939
20.029872	706.124233	12.706944
20.241765	701.972744	12.711949
20.046435	709.287080	12.716954
19.958912	701.551278	12.721959
19.918931	705.818318	12.726963
20.053446	695.944828	12.731968
19.830060	704.986620	12.736973
20.384340	725.817042	12.741978
20.226169	726.260323	12.746983
20.205866	708.745212	12.751987
20.027602	708.737491	12.756992
20.194277	706.984102	12.761997
19.770265	707.348346	12.767002
20.557289	721.560391	12.772007
19.871841	717.641124	12.777011
20.362416	708.943343	12.782016
20.438446	711.065158	12.787021
20.304003	710.158597	12.792026
20.325614	706.992392	12.797031
20.254876	699.159288	12.802035
19.935224	708.852008	12.807040
20.824505	695.417688	12.812045
19.982921	717.363368	12.817050
20.143344	713.959747	12.822055
20.052428	713.838738	12.827059
20.355762	712.638405	12.832064
20.301256	703.074205	12.837069
20.296643	713.688966	12.842074
20.114786	714.182549	12.847079
20.233568	709.609839	12.852083
20.074290	707.406129	12.857088
20.127580	714.322023	12.862093
19.634550	715.454285	12.867098
19.881511	706.983035	12.872103
19.787531	715.829136	12.877107
20.078598	723.946714	12.882112
20.128645	720.328861	12.887117
20.049567	717.100646	12.892122
20.098407	717.164736	12.897127
20.076626	719.807615	12.902131
19.933974	720.835892	12.907136
19.949965	710.117832	12.912141
19.621617	713.215709	12.917146
19.861558	717.852097	12.922151
20.220946	741.708546	12.927155
20.372427	741.966810	12.932160
20.439431	726.869650	12.937165
20.016749	725.218142	12.942170
19.880080	719.034944	12.947175
19.918243	719.830147	12.952179
20.265484	725.016393	12.957184
20.344483	730.672819	12.962189
20.113699	728.061001	12.967194
20.412398	712.874857	12.972199
19.883361	719.130564	12.977203
19.709233	715.328460	12.982208
20.286490	728.532292	12.987213
20.151394	723.672821	12.992218
20.186778	728.679338	12.997223
20.138848	728.306233	13.002227
19.802610	718.024428	13.007232
20.278301	726.933444	13.012237
20.257931	732.380193	13.017242
20.330411	729.376197	13.022247
20.147126	722.765150	13.027251
19.867436	718.871851	13.032256
20.226856	719.816108	13.037261
19.993191	722.187612	13.042266
20.057424	718.085692	13.047271
20.028259	730.679704	13.052275
20.482249	734.778072	13.057280
20.294426	720.212831	13.062285
19.899529	723.424625	13.067290
19.966850	715.261169	13.072295
20.226397	719.851061	13.077299
20.125893	724.988070	13.082304
20.139295	712.014373	13.087309
20.412165	711.247871	13.092314
20.081925	713.503089	13.097319
20.301788	725.081939	13.102323
20.536846	721.671143	13.107328
20.583072	718.281791	13.112333
20.141234	724.029171	13.117338
20.280825	728.090153	13.122343
20.375563	727.199871	13.127347
20.361188	718.620470	13.132352
20.409739	720.978504	13.137357
20.155931	723.591364	13.142362
19.994900	712.922038	13.147367
20.482637	717.792531	13.152371
20.246823	708.591591	13.157376
20.082186	693.498292	13.162381
20.104780	703.671060	13.167386
20.131553	692.064173	13.172391
20.066523	701.535699	13.177395
19.918998	694.499453	13.182400
20.111687	699.672490	13.187405
20.061610	726.033209	13.192410
20.083234	723.463143	13.197415
20.226365	726.487403	13.202419
20.258718	722.492289	13.207424
20.241387	706.650802	13.212429
19.849699	704.383226	13.217434
20.417202	702.707058	13.222439
20.280184	701.377456	13.227443
20.037204	689.439033	13.232448
20.406737	691.126856	13.237453
20.040389	698.042645	13.242458
20.207602	696.091244	13.247463
20.252795	699.210762	13.252467
20.232481	692.214946	13.257472
20.137583	694.418431	13.262477
19.820117	706.362114	13.267482
19.811470	686.015060	13.272487
20.134335	691.060088	13.277491
20.196276	697.843695	13.282496
19.990579	696.150486	13.287501
19.699037	703.417868	13.292506
20.629976	717.692908	13.297511
20.539526	710.685402	13.302515
20.287308	707.800224	13.307520
20.542431	703.647360	13.312525
20.198563	705.542016	13.317530
20.451431	704.187292	13.322535
20.173630	700.518433	13.327539
19.953546	701.468376	13.332544
20.326770	699.417090	13.337549
19.756018	697.201731	13.342554
20.078328	695.055267	13.347559
20.121357	698.981029	13.352563
19.780848	702.585516	13.357568
20.322043	693.191265	13.362573
20.186077	699.537250	13.367578
20.067426	696.331122	13.372583
20.174214	704.987485	13.377587
19.964875	703.250697	13.382592
20.073579	704.679684	13.387597
19.835761	711.490605	13.392602
20.029338	697.398405	13.397607
19.642552	705.005862	13.402611
19.792811	706.496037	13.407616
19.886739	716.101507	13.412621
19.849134	734.069273	13.417626
20.170772	734.176594	13.422631
20.239076	739.971149	13.427635
20.072923	738.297651	13.432640
20.455942	737.470998	13.437645
20.321817	740.408581	13.442650
20.336932	719.896036	13.447655
20.092273	717.299838	13.452659
19.970627	707.509778	13.457664
19.951212	706.566734	13.462669
19.991629	724.337523	13.467674
20.273889	726.644878	13.472679
20.431838	729.461751	13.477683
19.848202	723.285178	13.482688
20.175754	714.433604	13.487693
19.855157	714.436757	13.492698
20.304138	725.506722	13.497703
20.285752	739.069729	13.502707
19.913650	736.167394	13.507712
20.308863	728.604555	13.512717
19.998873	723.658638	13.517722
20.339363	723.626533	13.522727
20.515043	718.114254	13.527731
20.362668	715.955966	13.532736
20.501947	710.604841	13.537741
19.924626	717.104813	13.542746
20.378883	706.587328	13.547751
19.960860	703.438409	13.552755
20.021575	716.406040	13.557760
20.171931	709.101482	13.562765
19.874341	713.790483	13.567770
20.012840	712.092842	13.572775
20.128651	713.875544	13.577779
20.314172	712.608050	13.582784
20.156079	711.698164	13.587789
20.157555	715.558800	13.592794
20.000570	709.262140	13.597799
20.304274	713.680968	13.602803
19.959944	713.187175	13.607808
20.236410	705.118113	13.612813
19.902436	707.470917	13.617818
20.131915	709.422376	13.622823
20.298492	717.086675	13.627827
19.930669	715.732377	13.632832
20.083518	715.771993	13.637837
19.907624	713.410068	13.642842
20.127709	714.147079	13.647847
20.199409	714.179135	13.652851
20.136647	707.854043	13.657856
20.148494	710.213198	13.662861
19.921173	712.241457	13.667866
20.310401	712.511479	13.672871
20.169914	707.787715	13.677875
20.338629	710.357628	13.682880
20.387358	715.533917	13.687885
20.093030	721.460426	13.692890
20.331378	714.916978	13.697895
20.418881	725.606950	13.702899
20.196499	719.533625	13.707904
20.196350	712.879181	13.712909
20.158507	714.523948	13.717914
20.513880	717.277001	13.722919
20.343091	717.066219	13.727923
20.097253	719.344249	13.732928
20.468696	721.845557	13.737933
20.278815	707.928058	13.742938
20.285265	695.601307	13.747943
20.246210	690.430822	13.752947
19.657345	684.147069	13.757952
19.890675	685.824284	13.762957
20.162910	710.117245	13.767962
20.390907	710.607754	13.772967
20.205363	696.297665	13.777971
19.753197	693.595782	13.782976
19.986587	706.923043	13.787981
20.091981	713.366958	13.792986
19.941400	712.198017	13.797991
20.186975	716.331198	13.802995
19.887275	713.713815	13.808000
19.905766	714.655672	13.813005
20.004123	718.784735	13.818010
20.454419	708.091245	13.823015
20.361544	718.351044	13.828019
20.204591	715.714835	13.833024
20.333393	710.789621	13.838029
19.778046	722.924237	13.843034
20.309215	717.598134	13.848039
20.298376	720.962370	13.853043
19.978733	726.317276	13.858048
20.067171	723.232669	13.863053
19.997249	723.432407	13.868058
20.396288	723.047943	13.873063
20.405571	716.315503	13.878067
20.149853	710.702493	13.883072
20.140922	692.638332	13.888077
20.082986	701.246842	13.893082
19.963085	691.902045	13.898087
20.036991	700.949251	13.903091
19.942368	708.914639	13.908096
20.539927	719.164465	13.913101
20.347974	707.766720	13.918106
20.366836	695.788895	13.923111
20.047642	697.374446	13.928115
20.024127	705.733806	13.933120
20.400408	700.903178	13.938125
20.061063	703.979151	13.943130
20.121209	694.946290	13.948135
20.376910	701.657202	13.953139
19.955779	701.364912	13.958144
19.783018	699.198839	13.963149
19.701728	703.029301	13.968154
20.005054	693.189607	13.973159
20.120316	695.186092	13.978163
19.988051	726.819556	13.983168
20.405174	720.662370	13.988173
19.789710	724.402977	13.993178
19.927104	724.378031	13.998183
20.285972	723.686919	14.003187
20.253145	722.057607	14.008192
20.599957	715.029134	14.013210
20.015415	708.805783	14.018227
20.122444	698.795062	14.023245
20.132459	702.649989	14.028263
19.672753	705.121591	14.033280
20.393870	707.645540	14.038298
20.243776	722.352734	14.043315
20.350055	723.340317	14.048333
20.350441	730.691389	14.053351
20.221279	730.940208	14.058368
20.435599	726.623431	14.063386
20.099681	727.665811	14.068403
20.367851	726.194803	14.073421
20.404416	728.033532	14.078439
20.122590	728.471873	14.083456
20.416840	725.080692	14.088474
20.541135	732.052552	14.093491
20.245817	733.827807	14.098509
20.585304	730.307495	14.103527
20.382871	734.949822	14.108544
20.530570	727.416492	14.113562
20.344475	733.190404	14.118579
20.595956	730.502918	14.123597
20.692495	732.073310	14.128615
20.652937	731.533094	14.133632
20.707697	734.157036	14.138650
20.391362	725.863983	14.143667
20.178456	729.118947	14.148685
20.556165	732.400053	14.153703
20.282653	733.800582	14.158720
20.673760	727.259586	14.163738
20.407536	728.710077	14.168755
20.275959	722.758193	14.173773
20.520951	728.670208	14.178791
20.303721	736.010371	14.183808
20.682099	745.674945	14.188826
20.932850	759.504174	14.193843
20.868536	753.329969	14.198861
20.831186	762.387580	14.203879
20.921874	766.043247	14.208896
21.106342	755.803836	14.213914
20.775452	744.911212	14.218931
20.692007	730.744872	14.223949
20.833156	744.229758	14.228967
21.277468	764.933959	14.233984
21.419789	749.525823	14.239002
20.700873	743.507940	14.244019
20.812860	737.079886	14.249037
20.918801	742.893744	14.254055
20.649127	748.954709	14.259072
21.093002	752.447858	14.264090
20.912020	765.881105	14.269107
21.088276	769.317051	14.274125
21.181155	769.037294	14.279143
20.737299	774.606932	14.284160
21.306324	767.829107	14.289178
21.038027	771.186513	14.294195
21.186829	763.215671	14.299213
21.257032	772.024103	14.304231
21.033697	775.053430	14.309248
21.357266	771.000798	14.314266
21.056450	771.241601	14.319283
21.252761	763.396894	14.324301
21.296455	767.995256	14.329319
20.968774	775.043156	14.334336
21.101140	772.251961	14.339354
21.377886	770.116525	14.344371
20.967386	778.765667	14.349389
20.897827	774.376958	14.354407
20.884109	777.827475	14.359424
21.275955	773.867776	14.364442
21.314562	783.091831	14.369459
21.339631	794.338683	14.374477
21.742786	794.200569	14.379495
21.412585	809.380187	14.384512
21.447296	789.991949	14.389530
21.480600	789.993838	14.394547
21.517577	794.907897	14.399565
21.583733	791.975455	14.404583
21.421259	800.168969	14.409600
21.725714	798.577332	14.414618
21.350049	800.669015	14.419635
21.392814	808.523834	14.424653
21.829749	798.499754	14.429671
21.764669	808.277571	14.434688
21.765839	802.730790	14.439706
21.327911	801.780609	14.444723
21.484388	804.368676	14.449741
21.632363	797.650914	14.454759
21.630304	800.695292	14.459776
21.994498	797.957569	14.464794
21.604817	795.399862	14.469811
21.633014	795.127275	14.474829
22.131367	793.739889	14.479847
21.897936	797.888510	14.484864
21.941951	799.534142	14.489882
22.070716	807.132202	14.494899
21.639993	805.125328	14.499917
21.738209	792.445628	14.504935
21.511403	798.266959	14.509952
21.891674	797.056502	14.514970
22.039930	798.542357	14.519987
21.963962	805.711368	14.525005
21.723241	803.648234	14.530023
21.590859	811.239968	14.535040
21.826913	824.534392	14.540058
22.301897	825.891058	14.545075
22.446781	826.323482	14.550093
22.492565	830.837370	14.555111
22.306234	826.486146	14.560128
22.424574	800.572740	14.565146
22.334347	802.227985	14.570163
22.045771	798.712658	14.575181
22.460403	798.446080	14.580199
22.116010	801.226508	14.585216
22.044412	799.309441	14.590234
22.419445	801.722644	14.595251
21.973260	792.942156	14.600269
22.415946	800.708016	14.605287
22.311515	802.929480	14.610304
22.509939	801.130588	14.615322
22.524665	800.312713	14.620339
22.408750	801.444284	14.625357
22.414791	792.214914	14.630375
22.165861	800.122544	14.635392
22.279191	815.698637	14.640410
22.816885	815.108824	14.645427
22.553341	820.504997	14.650445
22.532197	803.158084	14.655463
22.495015	814.425892	14.660480
22.525411	807.123597	14.665498
22.703851	810.335039	14.670515
22.611241	812.517650	14.675533
22.823133	800.176118	14.680551
22.818371	798.685710	14.685568
22.750755	798.746955	14.690586
22.971545	793.261108	14.695603
22.720365	804.577197	14.700621
22.514164	794.584906	14.705639
22.591469	796.332985	14.710656
22.549228	791.228091	14.715674
22.866815	808.571213	14.720691
22.863618	813.954961	14.725709
23.001369	801.158831	14.730727
22.559291	799.096352	14.735744
22.864961	811.074782	14.740762
23.287949	814.176433	14.745779
23.125547	811.164031	14.750797
23.085480	802.150443	14.755815
22.882422	805.269353	14.760832
22.815432	799.450288	14.765850
22.819083	798.773399	14.770867
22.406446	810.037376	14.775885
23.113206	817.078406	14.780903
22.987756	830.805676	14.785920
22.909443	831.665398	14.790938
23.284357	830.565123	14.795955
23.161152	832.261812	14.800973
23.139221	833.365811	14.805991
23.010733	830.124617	14.811008
23.446483	829.298582	14.816026
23.311767	818.852047	14.821043
22.883592	825.307213	14.826061
23.166624	827.826334	14.831079
22.986950	825.714920	14.836096
23.176746	827.130443	14.841114
23.273951	821.530584	14.846131
23.161118	831.548851	14.851149
23.263527	826.076366	14.856167
23.300549	832.772746	14.861184
22.979678	827.029556	14.866202
23.360669	828.431889	14.871219
23.065286	835.226118	14.876237
23.354417	826.657894	14.881255
23.670911	828.402436	14.886272
23.246107	823.585072	14.891290
23.351885	833.962534	14.896307
23.581679	852.433460	14.901325
23.764718	849.295166	14.906343
23.239552	842.455858	14.911360
23.656958	846.619458	14.916378
23.882125	856.076510	14.921395
23.307881	857.649289	14.926413
23.571063	856.348959	14.931431
23.654070	855.005003	14.936448
23.920607	854.784854	14.941466
23.999757	855.586429	14.946483
23.636188	848.586058	14.951501
23.873094	841.489920	14.956519
23.766056	838.414411	14.961536
23.768782	840.370240	14.966554
24.044642	838.352131	14.971571
23.582896	836.499644	14.976589
23.900551	837.102723	14.981607
23.761473	855.453153	14.986624
23.644488	852.040225	14.991642
23.736037	848.230653	14.996659
24.118346	850.104707	15.001677
24.123668	847.511519	15.006695
23.857249	852.330049	15.011712
23.970181	852.486773	15.016730
24.438783	854.893714	15.021747
24.252256	860.697634	15.026765
24.054394	852.859115	15.031783
24.335304	850.586144	15.036800
24.172893	846.970454	15.041818
24.317142	849.600594	15.046835
24.024227	844.024406	15.051853
24.256355	835.539204	15.056871
24.095574	846.093688	15.061888
24.318878	849.128875	15.066906
24.544704	844.029974	15.071923
23.877981	850.741072	15.076941
24.147905	853.401507	15.081959
24.274015	855.780486	15.086976
24.080462	853.123844	15.091994
24.505657	857.817911	15.097011
24.111929	859.531007	15.102029
24.173839	849.473106	15.107047
24.214535	846.904952	15.112064
24.214407	853.185677	15.117082
24.566301	840.127260	15.122099
24.281643	846.076605	15.127117
24.301978	845.389974	15.132135
24.524201	851.296232	15.137152
24.406274	848.693599	15.142170
24.638848	842.615944	15.147187
24.468189	852.111742	15.152205
24.474459	843.768742	15.157223
24.646724	853.874480	15.162240
24.533314	858.602538	15.167258
24.946983	861.038692	15.172275
24.541747	849.986379	15.177293
24.495082	849.119302	15.182311
24.867527	865.325834	15.187328
25.028662	876.271036	15.192346
25.334375	867.854307	15.197363
24.976773	861.670202	15.202381
24.853471	848.103163	15.207399
24.936999	841.656006	15.212416
24.465236	846.963482	15.217434
24.921222	837.055893	15.222451
24.688194	848.599579	15.227469
24.736870	847.499423	15.232487
25.116684	866.717257	15.237504
25.084141	865.408247	15.242522
25.320195	868.233756	15.247539
24.700441	866.024204	15.252557
25.040386	866.757442	15.257575
25.130466	878.734919	15.262592
24.774452	874.459511	15.267610
25.323799	874.101443	15.272627
25.339568	873.553971	15.277645
25.288480	878.771555	15.282663
25.393435	874.990514	15.287680
24.913650	877.658836	15.292698
25.117721	871.623469	15.297715
24.897020	878.049501	15.302733
24.912868	873.067453	15.307751
25.194052	874.696505	15.312768
25.043818	872.966583	15.317786
25.093000	878.496952	15.322803
25.306162	876.561987	15.327821
25.281226	877.288138	15.332839
25.474426	880.328920	15.337856
25.320089	876.803961	15.342874
25.366917	869.259904	15.347891
25.477400	889.768977	15.352909
25.637248	905.130098	15.357927
25.823447	897.209063	15.362944
25.574879	899.012275	15.367962
25.441117	880.338231	15.372979
25.607585	883.203157	15.377997
25.680638	890.778684	15.383015
25.885957	893.948890	15.388032
25.548448	883.821743	15.393050
25.796261	873.147411	15.398067
25.384578	882.953816	15.403085
25.540713	896.544997	15.408103
25.920488	895.486416	15.413120
25.941181	896.722840	15.418138
26.392419	895.249361	15.423155
25.799363	892.026403	15.428173
25.702823	877.356258	15.433191
25.927253	868.828217	15.438208
25.563710	874.724872	15.443226
26.201748	881.135072	15.448243
26.256620	892.837378	15.453261
26.034553	865.581236	15.458279
25.842975	860.544182	15.463296
25.736322	870.442722	15.468314
26.162116	876.701932	15.473331
25.858819	894.244860	15.478349
26.385556	896.100604	15.483367
26.477780	899.899998	15.488384
25.957405	890.716770	15.493402
26.229630	889.897936	15.498419
26.224797	900.226230	15.503437
26.114455	892.292716	15.508455
26.217358	887.307004	15.513472
26.250011	894.460307	15.518490
26.139897	896.658308	15.523507
26.348224	900.819875	15.528525
26.277088	894.500401	15.533543
26.427916	895.793938	15.538560
26.019085	903.742071	15.543578
26.353934	893.711398	15.548595
26.169760	900.877263	15.553613
26.165948	905.959895	15.558631
26.608333	898.177334	15.563648
26.099293	906.951598	15.568666
26.303705	908.415137	15.573683
26.341189	906.398857	15.578701
26.531146	895.250007	15.583719
26.680540	901.798715	15.588736
26.472871	910.663348	15.593754
26.998819	911.252874	15.598771
26.684003	906.800203	15.603789
26.337585	904.005116	15.608807
26.943338	909.412906	15.613824
26.768633	925.034269	15.618842
27.182768	922.460814	15.623859
26.840059	915.892833	15.628877
26.637942	918.194390	15.633895
26.658910	899.907796	15.638912
26.812691	925.080550	15.643930
27.106470	919.958986	15.648947
26.767085	922.530201	15.653965
27.079110	928.592851	15.658983
27.429656	910.191541	15.664000
27.069755	897.004340	15.669018
26.812761	896.778810	15.674035
26.682271	900.265284	15.679053
26.747896	916.630138	15.684071
27.084106	925.495343	15.689088
27.082471	931.594648	15.694106
27.555225	930.192457	15.699123
27.363980	925.265445	15.704141
27.138789	933.556344	15.709159
27.416988	919.376189	15.714176
27.011310	915.762313	15.719194
27.282033	920.919933	15.724211
27.336602	923.219880	15.729229
27.072226	933.562850	15.734247
27.108521	932.115433	15.739264
26.957343	928.733110	15.744282
27.313076	933.905493	15.749299
27.450483	929.032247	15.754317
27.495466	936.611488	15.759335
27.584886	930.484266	15.764352
27.507460	930.613146	15.769370
27.282424	934.355392	15.774387
27.590783	925.018729	15.779405
27.118541	926.723117	15.784423
27.647890	920.314152	15.789440
27.751603	925.198734	15.794458
27.551074	922.625780	15.799475
27.499234	933.296665	15.804493
27.571992	930.842152	15.809511
28.244428	920.896052	15.814528
27.489889	928.734947	15.819546
27.698339	922.234008	15.824563
27.817394	923.597113	15.829581
27.431583	922.546584	15.834599
27.471734	922.653566	15.839616
27.556046	931.046118	15.844634
27.964196	940.008403	15.849651
27.776556	946.259296	15.854669
27.599512	950.631786	15.859687
28.049486	943.068226	15.864704
28.262101	945.667816	15.869722
28.018507	951.023886	15.874739
28.526140	941.156755	15.879757
28.167205	950.540280	15.884775
28.502436	947.950302	15.889792
28.199645	944.996444	15.894810
28.052105	931.168911	15.899827
28.313521	931.940634	15.904845
27.996980	939.343144	15.909863
28.253437	932.220248	15.914880
28.428938	947.908482	15.919898
28.434174	942.980016	15.924915
28.471174	925.056580	15.929933
28.183534	927.499987	15.934951
28.405422	924.062097	15.939968
28.188140	924.682855	15.944986
28.646717	933.055831	15.950003
28.664870	920.884316	15.955021
28.414190	922.797984	15.960039
28.484715	914.482449	15.965056
27.959597	915.556590	15.970074
28.244304	937.743188	15.975091
28.527052	932.082231	15.980109
28.249662	942.415484	15.985127
28.642638	937.392144	15.990144
28.496566	949.690503	15.995162
28.634389	945.422044	16.000179
28.632646	941.207309	16.005197
28.033872	944.168340	16.010215
28.588351	944.066656	16.015232
28.465131	944.546564	16.020250
28.495582	941.478207	16.025267
28.837042	952.872931	16.030285
28.868680	967.728363	16.035303
29.291505	967.406991	16.040320
28.978709	955.571389	16.045338
29.116491	947.668275	16.050355
29.003258	938.562446	16.055373
28.781124	943.452598	16.060391
29.234450	940.677037	16.065408
28.842724	939.337999	16.070426
28.991483	936.375049	16.075443
29.195980	934.017507	16.080461
28.873671	935.364486	16.085479
29.135334	946.858453	16.090496
29.333792	966.595368	16.095514
29.413561	955.986317	16.100531
28.909150	936.158451	16.105549
29.209270	963.347462	16.110567
29.665705	961.412228	16.115584
29.088866	947.157619	16.120602
29.195549	951.856898	16.125619
29.722008	957.234880	16.130637
29.189918	952.838871	16.135655
29.423513	952.005745	16.140672
29.300592	964.975286	16.145690
29.131955	972.016006	16.150707
29.639181	967.705142	16.155725
29.432689	963.684299	16.160743
29.626882	965.229703	16.165760
29.424981	970.278666	16.170778
29.365234	971.356458	16.175795
29.684022	978.891266	16.180813
29.334573	975.745844	16.185831
29.603361	963.503644	16.190848
29.466866	967.454372	16.195866
28.945650	966.308239	16.200883
29.496984	969.744190	16.205901
29.656620	990.982568	16.210919
29.879652	985.197401	16.215936
29.776064	992.912845	16.220954
29.669684	995.612874	16.225971
29.786870	993.028562	16.230989
29.988347	1002.646013	16.236007
30.050111	997.128822	16.241024
30.101078	993.792899	16.246042
29.867995	993.079821	16.251059
30.557808	987.024354	16.256077
30.205016	995.103606	16.261095
30.319528	989.792734	16.266112
29.933263	974.010103	16.271130
30.359920	979.597504	16.276147
30.074976	966.238614	16.281165
29.942385	974.751521	16.286183
30.312774	983.000944	16.291200
30.559576	989.280886	16.296218
30.374319	978.355419	16.301235
30.466142	972.903446	16.306253
30.357223	969.588309	16.311271
30.416814	969.827478	16.316288
30.223370	966.376378	16.321306
30.244271	964.833093	16.326323
30.005550	975.127953	16.331341
30.224229	983.336290	16.336359
30.419271	986.678838	16.341376
30.446295	999.280771	16.346394
30.080974	997.991788	16.351411
30.502162	987.212638	16.356429
30.422341	998.980560	16.361447
30.342647	995.146349	16.366464
30.575964	1000.284794	16.371482
30.423104	990.198126	16.376499
30.763017	1008.875857	16.381517
30.999104	1014.132636	16.386535
30.845423	998.509523	16.391552
30.654494	996.793943	16.396570
30.422134	1007.927066	16.401587
31.152696	1009.784926	16.406605
30.756282	1024.784195	16.411623
31.026021	1025.281661	16.416640
31.250515	1018.519344	16.421658
31.323169	1018.073699	16.426675
31.032681	1000.784452	16.431693
30.637246	1004.440629	16.436711
31.103709	1008.890625	16.441728
31.537290	1010.773827	16.446746
31.104061	1005.739082	16.451763
31.140937	988.621807	16.456781
31.002422	991.931821	16.461799
31.318668	1009.488554	16.466816
31.430295	1012.864863	16.471834
31.298216	1006.423704	16.476851
31.177858	995.783618	16.481869
31.178528	1008.252902	16.486887
31.239799	1012.726622	16.491904
31.306030	999.826101	16.496922
31.298159	1015.372186	16.501939
31.298648	1004.693156	16.506957
31.371835	1017.001435	16.511975
31.505927	1014.075418	16.516992
31.553493	1013.428483	16.522010
31.345085	1014.772246	16.527027
32.026527	1003.537062	16.532045
31.833768	1011.371349	16.537063
31.726016	1009.367994	16.542080
31.841770	1010.805569	16.547098
31.602481	1008.396092	16.552115
31.895679	1007.868080	16.557133
32.050310	1015.736632	16.562151
31.904691	1010.701634	16.567168
31.807946	999.416736	16.572186
31.786903	1002.254961	16.577203
31.746139	1003.538164	16.582221
31.651567	1014.231655	16.587239
31.775843	1012.003306	16.592256
32.044225	1013.326086	16.597274
31.974852	1017.890647	16.602291
32.124524	1011.701082	16.607309
32.231539	1015.284204	16.612327
31.879268	1007.160324	16.617344
31.967251	1010.609620	16.622362
32.078246	1014.327396	16.627379
32.449686	1008.665636	16.632397
32.006973	1006.902904	16.637415
31.867240	1007.126670	16.642432
32.192605	1006.554985	16.647450
31.911564	1014.397062	16.652467
32.123751	1013.338459	16.657485
31.971851	1006.727419	16.662503
31.992208	1017.720352	16.667520
32.253831	1032.982001	16.672538
32.058861	1044.166607	16.677555
32.606653	1034.496728	16.682573
32.439951	1044.146972	16.687591
32.560894	1041.421258	16.692608
32.790626	1034.122453	16.697626
32.756388	1045.857972	16.702643
32.934598	1034.644032	16.707661
32.597762	1043.194273	16.712679
32.559476	1042.572041	16.717696
32.510410	1044.104337	16.722714
32.525878	1040.316289	16.727731
32.610829	1037.882623	16.732749
32.854685	1033.222040	16.737767
32.943543	1035.348213	16.742784
33.336129	1034.633666	16.747802
33.126879	1039.098626	16.752819
33.006312	1037.401708	16.757837
33.015780	1033.458880	16.762855
33.163313	1028.045194	16.767872
33.039146	1026.872699	16.772890
32.709240	1034.783931	16.777907
33.133498	1029.843665	16.782925
33.029156	1033.766472	16.787943
32.843178	1038.105018	16.792960
32.971627	1033.252043	16.797978
32.615060	1039.647115	16.802995
32.921991	1031.875076	16.808013
32.960591	1046.661833	16.813031
32.881056	1053.679729	16.818048
33.435004	1066.740408	16.823066
33.430073	1075.983390	16.828083
33.317119	1070.765399	16.833101
33.174073	1071.076216	16.838119
32.930786	1060.543783	16.843136
33.386113	1060.304535	16.848154
33.188432	1063.882779	16.853171
33.575450	1058.661349	16.858189
33.693059	1058.523943	16.863207
33.533479	1058.614014	16.868224
33.639835	1060.116805	16.873242
33.563348	1065.597284	16.878259
33.455309	1065.874988	16.883277
33.641061	1057.413572	16.888295
33.488893	1059.833821	16.893312
33.784365	1062.029297	16.898330
33.930164	1081.434973	16.903347
34.137472	1074.213661	16.908365
33.788787	1068.660438	16.913383
33.480772	1061.276700	16.918400
34.214607	1069.295166	16.923418
34.007176	1085.794214	16.928435
34.113854	1086.809289	16.933453
34.168281	1083.164462	16.938471
33.789712	1084.675378	16.943488
34.363952	1083.021020	16.948506
34.210937	1090.421909	16.953523
34.142468	1077.589209	16.958541
34.248171	1073.301453	16.963559
34.292181	1087.905695	16.968576
34.793484	1074.105898	16.973594
34.107943	1061.792437	16.978611
34.140876	1062.359921	16.983629
34.257638	1062.890439	16.988647
34.374345	1081.378121	16.993664
34.561415	1090.028100	16.998682
34.594845	1096.007830	17.003699
34.543079	1078.825144	17.008717
34.435074	1077.818390	17.013735
34.619441	1080.085863	17.018752
34.838609	1072.154756	17.023770
34.721640	1061.922305	17.028787
34.464681	1058.541091	17.033805
34.448816	1063.394452	17.038823
34.705903	1080.606756	17.043840
34.842020	1080.781022	17.048858
34.806829	1084.097388	17.053875
35.118466	1082.145904	17.058893
34.856029	1069.188409	17.063911
34.704856	1070.098306	17.068928
34.699694	1059.350920	17.073946
34.700261	1085.536307	17.078963
34.693734	1083.638713	17.083981
35.205436	1086.751446	17.088999
34.870116	1087.449240	17.094016
35.191870	1091.127916	17.099034
35.188855	1090.071381	17.104051
34.968406	1089.927326	17.109069
35.207083	1079.559486	17.114087
35.005472	1089.704567	17.119104
35.330050	1081.707090	17.124122
35.039660	1087.678684	17.129139
35.030505	1085.447221	17.134157
35.039730	1089.885218	17.139175
34.734481	1093.099143	17.144192
35.087361	1090.297102	17.149210
35.277702	1111.251530	17.154227
35.504860	1110.940913	17.159245
35.609202	1115.498250	17.164263
35.518260	1108.361457	17.169280
35.768766	1107.808788	17.174298
35.636158	1104.012877	17.179315
35.735564	1103.102824	17.184333
36.039564	1107.179976	17.189351
35.397112	1093.057603	17.194368
35.774100	1092.564992	17.199386
35.693098	1104.884566	17.204403
35.827759	1107.266943	17.209421
35.704899	1108.424027	17.214439
35.612125	1108.994257	17.219456
35.782676	1102.610189	17.224474
35.670112	1104.195093	17.229491
35.923593	1111.463517	17.234509
35.857339	1104.520216	17.239527
35.852428	1105.720627	17.244544
35.736254	1101.063170	17.249562
35.770594	1106.280582	17.254579
35.939659	1104.614546	17.259597
36.143386	1098.509137	17.264615
35.773959	1104.034777	17.269632
35.807866	1108.059045	17.274650
36.315592	1123.367275	17.279667
36.187631	1121.157901	17.284685
36.486781	1126.419608	17.289703
36.211095	1124.285707	17.294720
36.511855	1122.793732	17.299738
36.577839	1125.062788	17.304755
36.432109	1131.284265	17.309773
36.825898	1121.981833	17.314791
36.563892	1134.254003	17.319808
36.565476	1118.215863	17.324826
36.502622	1120.914478	17.329843
36.768359	1120.095095	17.334861
36.753546	1121.504739	17.339879
36.628704	1125.664449	17.344896
36.746497	1125.251716	17.349914
36.854215	1120.995087	17.354931
36.920007	1110.611538	17.359949
36.972658	1110.275266	17.364967
36.969250	1119.061827	17.369984
37.163994	1117.322477	17.375002
37.139684	1120.794428	17.380019
36.823731	1112.481427	17.385037
37.239831	1108.824532	17.390055
37.125187	1114.175040	17.395072
36.858325	1098.668976	17.400090
36.730133	1104.822360	17.405107
36.864228	1112.379616	17.410125
37.231283	1118.927531	17.415143
37.100490	1127.172021	17.420160
37.215936	1116.756164	17.425178
37.252718	1112.726369	17.430195
37.302714	1118.878870	17.435213
37.298008	1113.604271	17.440231
37.418386	1122.220073	17.445248
37.177921	1114.797218	17.450266
37.147128	1117.613423	17.455283
37.211514	1119.837899	17.460301
37.267249	1120.376579	17.465319
37.243129	1137.120960	17.470336
37.849514	1147.191489	17.475354
37.848563	1154.720751	17.480371
37.594558	1150.551693	17.485389
37.844101	1135.438315	17.490407
37.534205	1140.753901	17.495424
37.638334	1143.786135	17.500442
37.775956	1144.766390	17.505459
37.940459	1154.330061	17.510477
37.752760	1149.555786	17.515495
37.748177	1151.491586	17.520512
37.996857	1144.466574	17.525530
37.905562	1139.711536	17.530547
37.546264	1154.538266	17.535565
37.790555	1146.766718	17.540583
37.796846	1143.938927	17.545600
37.877686	1145.274326	17.550618
37.726933	1151.090745	17.555635
38.127683	1166.998140	17.560653
38.391613	1163.372580	17.565671
38.116324	1178.507641	17.570688
38.352717	1172.841401	17.575706
38.575232	1185.737955	17.580723
38.229272	1177.270816	17.585741
38.763594	1171.404467	17.590759
38.941815	1173.747659	17.595776
38.486548	1158.303042	17.600794
38.572937	1149.382335	17.605811
38.029491	1152.277949	17.610829
38.546415	1157.977660	17.615847
38.589037	1169.755294	17.620864
38.761918	1172.792301	17.625882
38.897518	1173.756362	17.630899
38.445453	1181.199485	17.635917
38.914966	1179.836332	17.640935
38.760664	1184.246951	17.645952
38.924250	1183.491051	17.650970
38.685399	1187.795598	17.655987
38.647901	1178.579219	17.661005
38.803448	1168.429868	17.666023
38.789944	1179.567545	17.671040
39.005531	1174.606239	17.676058
38.889733	1176.772152	17.681075
38.686687	1186.001180	17.686093
39.089975	1177.726812	17.691111
38.947366	1177.365834	17.696128
39.167497	1170.451550	17.701146
39.231926	1184.325059	17.706163
39.365452	1189.665904	17.711181
39.683398	1189.266083	17.716199
39.419879	1191.494099	17.721216
39.242049	1184.706989	17.726234
39.405842	1173.160166	17.731251
39.189378	1185.458151	17.736269
39.489820	1198.019796	17.741287
39.663432	1203.647642	17.746304
39.603488	1207.482399	17.751322
39.611432	1205.232459	17.756339
39.349811	1206.433705	17.761357
39.510954	1204.448789	17.766375
39.336260	1209.552488	17.771392
39.265969	1208.107098	17.776410
39.663601	1205.321495	17.781427
39.599289	1207.760792	17.786445
39.589159	1211.937627	17.791463
39.699667	1217.017866	17.796480
39.864605	1226.544547	17.801498
40.345264	1225.560311	17.806515
40.567886	1221.655801	17.811533
40.585015	1199.324912	17.816551
40.293988	1192.684062	17.821568
40.473043	1188.834489	17.826586
40.580164	1183.637205	17.831603
40.251076	1188.434376	17.836621
40.538401	1175.258535	17.841639
40.541730	1188.013859	17.846656
40.400836	1183.818886	17.851674
40.444899	1183.552413	17.856691
39.918035	1190.900497	17.861709
40.400564	1180.302560	17.866727
40.341833	1184.764009	17.871744
40.352522	1182.670162	17.876762
40.512854	1183.764782	17.881779
40.113717	1189.290473	17.886797
40.299798	1185.890483	17.891815
40.694890	1188.807104	17.896832
40.602477	1194.371974	17.901850
40.737622	1207.123596	17.906867
40.792698	1212.362909	17.911885
41.128681	1204.981789	17.916903
40.864852	1204.592949	17.921920
40.941692	1198.430652	17.926938
40.831411	1180.521738	17.931955
41.080224	1201.659681	17.936973
41.020518	1205.748459	17.941991
40.769596	1201.213928	17.947008
40.801540	1203.900586	17.952026
41.154684	1205.653490	17.957043
40.747032	1206.200791	17.962061
41.425823	1199.667979	17.967079
40.924482	1199.776374	17.972096
40.923157	1212.803040	17.977114
41.090012	1199.084783	17.982131
41.246531	1204.108126	17.987149
41.380794	1197.238987	17.992167
41.436545	1204.537420	17.997184
41.403954	1207.610350	18.002202
41.515372	1208.848850	18.007219
41.387826	1220.798393	18.012237
41.825953	1222.621908	18.017255
41.850976	1222.233407	18.022272
41.607631	1211.765371	18.027290
41.926759	1199.103572	18.032307
41.575676	1205.783363	18.037325
41.689700	1220.951553	18.042343
41.507574	1231.147111	18.047360
41.597482	1232.923910	18.052378
41.645535	1237.707356	18.057395
41.596957	1239.730414	18.062413
41.929527	1228.892857	18.067431
41.758522	1237.032916	18.072448
41.793940	1240.620435	18.077466
41.827365	1240.446113	18.082483
41.808110	1240.572011	18.087501
42.118272	1252.591781	18.092519
42.281084	1259.177839	18.097536
42.438016	1254.949505	18.102554
42.574210	1253.785807	18.107571
42.224824	1264.672715	18.112589
42.519721	1261.605377	18.117607
42.471661	1259.759218	18.122624
42.499898	1257.583905	18.127642
42.695720	1252.374022	18.132659
42.403273	1259.589579	18.137677
42.587794	1257.941513	18.142695
42.519630	1259.434403	18.147712
42.360844	1262.620286	18.152730
42.783183	1247.686888	18.157747
42.550530	1259.234770	18.162765
42.510096	1255.696271	18.167783
42.762805	1261.073982	18.172800
42.589464	1258.572927	18.177818
42.621223	1251.677635	18.182835
42.730772	1256.982214	18.187853
42.836261	1259.809748	18.192871
42.706021	1273.372231	18.197888
42.885018	1295.505444	18.202906
43.665935	1295.139544	18.207923
42.880854	1297.962815	18.212941
43.227522	1298.440158	18.217959
43.462080	1299.883199	18.222976
43.380945	1298.220076	18.227994
43.592223	1294.867957	18.233011
43.437169	1306.575760	18.238029
43.396331	1300.567478	18.243047
43.371470	1296.243060	18.248064
43.619205	1301.144129	18.253082
43.379795	1293.337953	18.258099
43.245778	1297.212863	18.263117
43.288362	1297.339910	18.268135
43.680515	1294.859568	18.273152
43.500189	1295.544450	18.278170
43.770859	1290.354080	18.283187
43.438192	1292.547518	18.288205
43.557538	1293.488223	18.293223
43.424172	1293.294881	18.298240
43.509412	1299.679382	18.303258
43.874774	1303.274074	18.308275
43.416913	1309.610692	18.313293
43.735285	1309.196642	18.318311
44.053729	1311.758184	18.323328
44.090150	1319.372813	18.328346
44.344531	1312.357825	18.333363
44.413516	1323.031750	18.338381
44.173577	1311.092994	18.343399
44.119119	1317.091552	18.348416
43.966445	1322.110761	18.353434
44.205575	1314.777282	18.358451
44.209959	1316.072976	18.363469
44.486672	1315.289588	18.368487
44.306614	1322.346455	18.373504
44.211614	1328.746343	18.378522
44.545710	1342.729591	18.383539
44.631217	1351.793144	18.388557
44.659074	1345.878502	18.393575
44.553336	1348.204870	18.398592
44.587544	1345.611706	18.403610
45.069457	1350.151376	18.408627
44.765230	1343.768198	18.413645
44.449368	1347.620209	18.418663
44.927525	1351.067139	18.423680
44.912016	1353.530140	18.428698
44.984413	1343.623609	18.433715
44.745320	1343.963906	18.438733
45.055221	1338.512413	18.443751
45.132167	1344.522274	18.448768
44.904171	1350.238612	18.453786
45.070614	1336.536023	18.458803
44.757278	1348.887350	18.463821
44.790938	1360.685445	18.468839
45.326558	1365.219701	18.473856
45.091389	1376.258375	18.478874
45.314486	1373.495072	18.483891
45.300103	1373.635924	18.488909
45.384382	1378.397121	18.493927
45.406166	1367.505200	18.498944
45.550210	1382.192891	18.503962
45.764589	1373.530084	18.508979
45.502569	1379.017459	18.513997
45.823783	1371.839974	18.519015
45.613223	1369.013688	18.524032
45.396024	1373.166173	18.529050
45.663697	1366.974157	18.534067
45.687151	1370.812960	18.539085
45.855847	1394.997783	18.544103
46.133612	1402.489016	18.549120
45.800235	1406.365072	18.554138
46.345153	1399.284042	18.559155
46.043747	1404.651069	18.564173
45.763896	1403.249306	18.569191
46.066078	1403.333380	18.574208
46.003058	1409.975188	18.579226
46.162841	1406.980497	18.584243
46.274885	1403.578893	18.589261
46.366212	1399.512003	18.594279
46.399390	1400.946269	18.599296
46.090367	1407.374032	18.604314
46.431212	1399.426490	18.609331
46.612984	1411.197858	18.614349
46.503360	1405.849430	18.619367
46.474104	1405.099103	18.624384
46.277773	1414.000774	18.629402
46.743942	1420.210523	18.634419
47.054924	1434.088997	18.639437
46.817246	1438.443771	18.644455
47.101278	1429.660488	18.649472
46.740467	1451.060412	18.654490
46.984596	1436.776643	18.659507
47.026125	1429.874203	18.664525
46.865750	1434.842764	18.669543
47.074155	1425.989739	18.674560
46.922662	1434.145674	18.679578
46.939710	1434.744810	18.684595
46.949425	1429.194854	18.689613
46.906128	1425.062117	18.694631
47.003834	1419.344749	18.699648
46.812007	1438.064576	18.704666
47.148818	1436.848418	18.709683
47.383780	1456.798060	18.714701
47.467392	1464.421757	18.719719
47.573943	1455.782390	18.724736
47.192526	1460.318197	18.729754
47.682959	1455.043954	18.734771
47.701253	1453.139993	18.739789
47.461143	1460.560465	18.744807
47.668614	1452.507526	18.749824
47.660136	1462.193377	18.754842
47.629756	1455.749170	18.759859
48.064315	1451.914628	18.764877
47.674365	1460.131418	18.769895
48.006423	1457.489160	18.774912
47.924449	1455.244869	18.779930
47.838147	1449.693700	18.784947
47.591167	1460.127082	18.789965
48.221146	1468.424269	18.794983
48.271500	1474.657095	18.800000
48.290332	1486.117067	18.805018
48.274334	1478.840713	18.810035
48.463037	1481.347465	18.815053
48.429407	1481.677022	18.820071
48.469245	1477.953406	18.825088
48.721662	1477.007916	18.830106
48.741403	1467.980444	18.835123
48.712176	1481.364188	18.840141
48.543480	1480.444169	18.845159
48.782481	1476.402475	18.850176
48.574228	1483.020283	18.855194
48.762118	1483.676339	18.860211
49.078350	1483.441967	18.865229
48.602578	1479.903623	18.870247
49.288472	1476.230356	18.875264
48.874683	1477.408696	18.880282
48.918334	1480.237483	18.885299
48.874968	1481.756330	18.890317
48.557502	1476.925557	18.895335
48.819208	1469.305232	18.900352
48.786677	1479.064149	18.905370
48.924876	1476.722602	18.910387
48.979636	1478.745730	18.915405
49.032924	1498.412130	18.920423
49.314338	1510.246346	18.925440
49.319600	1509.595124	18.930458
49.376655	1509.991237	18.935475
49.566506	1507.061735	18.940493
49.295647	1507.437779	18.945511
49.501845	1501.932758	18.950528
49.679044	1508.926446	18.955546
49.311732	1509.960510	18.960563
49.708592	1506.538630	18.965581
49.821646	1508.392790	18.970599
49.805497	1503.194600	18.975616
49.736238	1517.435844	18.980634
49.793031	1512.065556	18.985651
49.677832	1509.609459	18.990669
49.568732	1521.956676	18.995687
49.932795	1533.706937	19.000704
50.013609	1538.174557	19.005722
50.103205	1536.734311	19.010739
50.251683	1531.765497	19.015757
49.850715	1540.637740	19.020775
50.197581	1531.595814	19.025792
50.350109	1537.751805	19.030810
50.367847	1533.609303	19.035827
50.339661	1525.689084	19.040845
50.136133	1536.239870	19.045863
50.441481	1525.993228	19.050880
50.426108	1539.344926	19.055898
50.953915	1543.422693	19.060915
50.992026	1531.220741	19.065933
50.572692	1529.080583	19.070951
50.611904	1525.071525	19.075968
50.973057	1541.236567	19.080986
51.145145	1535.635504	19.086003
50.919015	1533.579375	19.091021
50.867285	1528.659796	19.096039
51.277555	1527.119642	19.101056
51.097110	1530.434890	19.106074
50.825341	1532.800350	19.111091
51.033673	1544.409488	19.116109
51.067142	1555.883698	19.121127
51.255398	1549.211869	19.126144
51.469236	1561.724715	19.131162
51.319462	1561.105296	19.136179
51.532880	1550.213353	19.141197
51.355235	1559.148314	19.146215
51.507304	1549.357937	19.151232
51.545394	1550.749747	19.156250
51.377973	1554.057417	19.161267
51.705182	1547.680422	19.166285
51.453251	1557.590796	19.171303
51.670757	1550.368411	19.176320
51.428841	1556.201103	19.181338
51.503869	1549.710154	19.186355
52.076761	1561.924257	19.191373
51.925604	1581.892386	19.196391
52.060933	1579.589037	19.201408
52.220149	1586.094013	19.206426
52.136073	1595.659862	19.211443
51.943218	1582.022211	19.216461
52.129453	1578.413661	19.221479
52.242010	1582.254827	19.226496
52.001392	1588.585235	19.231514
51.815876	1585.404093	19.236531
51.996849	1576.204535	19.241549
52.172844	1586.261421	19.246567
52.338094	1602.117968	19.251584
52.393235	1608.498753	19.256602
52.776889	1614.621849	19.261619
52.753573	1613.500867	19.266637
52.825670	1623.780435	19.271655
52.683262	1610.763196	19.276672
52.510215	1610.265475	19.281690
52.682385	1605.157564	19.286707
53.030787	1608.595361	19.291725
53.003160	1605.991562	19.296743
52.546557	1603.594615	19.301760
52.874344	1606.825681	19.306778
52.699972	1605.868803	19.311795
53.082222	1608.570462	19.316813
52.930010	1613.490586	19.321831
53.196832	1599.979402	19.326848
53.515528	1607.124407	19.331866
53.262938	1610.629734	19.336883
53.241733	1606.926832	19.341901
53.609706	1626.948312	19.346919
53.861582	1626.838258	19.351936
53.649589	1613.834474	19.356954
53.361213	1607.449437	19.361971
53.391943	1613.211926	19.366989
53.466634	1621.410551	19.372007
53.901483	1625.796565	19.377024
53.738781	1625.648798	19.382042
53.926505	1631.499525	19.387059
54.145091	1623.880491	19.392077
53.841558	1625.046763	19.397095
54.017728	1616.348217	19.402112
54.256625	1615.559834	19.407130
54.306766	1625.201048	19.412147
54.086784	1620.602455	19.417165
54.210975	1620.999663	19.422183
54.385170	1617.758788	19.427200
54.335624	1616.309262	19.432218
53.954710	1614.505916	19.437235
54.502267	1610.873558	19.442253
53.974271	1622.936848	19.447271
53.996398	1615.225654	19.452288
54.488126	1632.685151	19.457306
54.540055	1637.151901	19.462323
54.737561	1638.663814	19.467341
54.604303	1645.070728	19.472359
54.847054	1642.143776	19.477376
54.902166	1649.186106	19.482394
54.536796	1657.118271	19.487411
54.831888	1642.698746	19.492429
54.674066	1648.717857	19.497447
54.648958	1645.379759	19.502464
54.991255	1656.841767	19.507482
54.947828	1675.711282	19.512499
55.228777	1674.090267	19.517517
55.107145	1680.142949	19.522535
55.448744	1674.168699	19.527552
55.305983	1674.012246	19.532570
55.221197	1677.870751	19.537587
55.399588	1668.275892	19.542605
55.729365	1674.666395	19.547623
55.692350	1683.204586	19.552640
55.822001	1674.713219	19.557658
55.630782	1670.301952	19.562675
55.778774	1676.557835	19.567693
55.787068	1674.395079	19.572711
55.568604	1671.191642	19.577728
55.712584	1668.731941	19.582746
55.464316	1674.929884	19.587763
56.174565	1683.108992	19.592781
56.221779	1691.022573	19.597799
55.919780	1681.226650	19.602816
56.168891	1681.612590	19.607834
56.263777	1699.287267	19.612851
56.505368	1702.437710	19.617869
56.261191	1712.915660	19.622887
56.429503	1709.346120	19.627904
56.420656	1704.795634	19.632922
56.482452	1706.643835	19.637939
56.631649	1705.529157	19.642957
56.913293	1706.558850	19.647975
56.696231	1711.093692	19.652992
56.550738	1705.827173	19.658010
56.336923	1708.524014	19.663027
56.514433	1705.196852	19.668045
56.561786	1707.967671	19.673063
56.709015	1700.587302	19.678080
56.870982	1702.933173	19.683098
56.910468	1712.075871	19.688115
57.153495	1711.201872	19.693133
57.148581	1727.202108	19.698151
57.052376	1726.165895	19.703168
57.075023	1720.750634	19.708186
56.887121	1724.255897	19.713203
57.073304	1718.886923	19.718221
57.097734	1721.866701	19.723239
57.303135	1716.353076	19.728256
57.098041	1723.096343	19.733274
57.529288	1740.354021	19.738291
57.559819	1748.886198	19.743309
57.755343	1744.776638	19.748327
57.581417	1751.764299	19.753344
57.757218	1744.248777	19.758362
57.847400	1752.407249	19.763379
57.979168	1740.096582	19.768397
57.939489	1748.969540	19.773415
58.074018	1749.119685	19.778432
58.530582	1744.052110	19.783450
58.403065	1744.221235	19.788467
58.166149	1738.760836	19.793485
58.412230	1746.209317	19.798503
58.289853	1746.605735	19.803520
58.695838	1728.164668	19.808538
58.648587	1723.852347	19.813555
59.016917	1720.545878	19.818573
59.400958	1718.710983	19.823591
59.560886	1702.573795	19.828608
59.355535	1677.644139	19.833626
59.142122	1680.958385	19.838643
59.161494	1672.491685	19.843661
59.318600	1669.876505	19.848679
58.788383	1656.918711	19.853696
58.818057	1653.186446	19.858714
58.934527	1654.807248	19.863731
59.000411	1664.641840	19.868749
59.144678	1670.383885	19.873767
58.767469	1679.591443	19.878784
59.275466	1673.044762	19.883802
58.841522	1675.123831	19.888819
59.357091	1673.131885	19.893837
58.978812	1677.795471	19.898855
59.140677	1674.751625	19.903872
59.165747	1673.063655	19.908890
58.814455	1686.157568	19.913907
59.815860	1692.781565	19.918925
59.675992	1704.263872	19.923943
59.393848	1704.445070	19.928960
59.848903	1704.753332	19.933978
59.661684	1713.999045	19.938995
59.685987	1706.691766	19.944013
59.579559	1710.662282	19.949031
59.525030	1716.759339	19.954048
59.952210	1721.695649	19.959066
59.945772	1736.305440	19.964083
60.318654	1732.888120	19.969101
60.049589	1736.061014	19.974119
59.951472	1740.385753	19.979136
60.052918	1738.262407	19.984154
60.036462	1740.924633	19.989171
60.025139	1738.276520	19.994189
60.534435	1748.878964	19.999207
60.337799	1757.596041	20.004224
60.770456	1763.486421	20.009242
60.702331	1772.304148	20.014259
60.873792	1771.369192	20.019277
60.715023	1767.715719	20.024295
60.694238	1771.388631	20.029312
61.130812	1768.262413	20.034330
60.818870	1769.199564	20.039347
60.814584	1766.369406	20.044365
61.191777	1772.453484	20.049383
61.148611	1774.895009	20.054400
60.938806	1773.355395	20.059418
61.063770	1771.357296	20.064435
60.904427	1785.834988	20.069453
61.255017	1786.605913	20.074471
61.357045	1794.698019	20.079488
61.586978	1795.180627	20.084506
61.217419	1802.035111	20.089523
61.368920	1796.204400	20.094541
61.593532	1785.637723	20.099559
61.658839	1792.649392	20.104576
61.790396	1788.677450	20.109594
61.704912	1800.984166	20.114611
62.035985	1809.751626	20.119629
62.430629	1818.375230	20.124647
61.754296	1813.474931	20.129664
61.917272	1806.285501	20.134682
62.032396	1820.431562	20.139699
61.915194	1822.227304	20.144717
62.103835	1816.842956	20.149735
62.411850	1819.241068	20.154752
62.658109	1820.267760	20.159770
62.297836	1824.761762	20.164787
62.522912	1818.426109	20.169805
62.669897	1816.972752	20.174823
62.324624	1828.949648	20.179840
62.691586	1819.714770	20.184858
62.537970	1819.964357	20.189875
62.465977	1827.244145	20.194893
62.879177	1845.978130	20.199911
63.053097	1853.652131	20.204928
63.232343	1840.926348	20.209946
63.315101	1852.941980	20.214963
63.069206	1846.893020	20.219981
63.040937	1842.177256	20.224999
62.940546	1848.093684	20.230016
63.158157	1849.987849	20.235034
63.328950	1846.371471	20.240051
63.139911	1846.038330	20.245069
62.982318	1847.997050	20.250087
63.447148	1867.421331	20.255104
63.599181	1873.116595	20.260122
63.465003	1871.656942	20.265139
63.549071	1874.905698	20.270157
64.092220	1865.062182	20.275175
63.473834	1883.322794	20.280192
64.061395	1875.238899	20.285210
63.894485	1876.516338	20.290227
63.953874	1871.534872	20.295245
63.989518	1868.006903	20.300263
64.161705	1874.609839	20.305280
64.235122	1864.405456	20.310298
64.014429	1889.217980	20.315315
63.929375	1896.558094	20.320333
64.443274	1897.742693	20.325351
64.330507	1902.064310	20.330368
64.522251	1896.299509	20.335386
64.539159	1892.798120	20.340403
64.361857	1901.806389	20.345421
64.774272	1901.394635	20.350439
64.109163	1909.677579	20.355456
64.744374	1916.947675	20.360474
65.026208	1933.746436	20.365491
65.071461	1926.756641	20.370509
65.322568	1916.129009	20.375527
65.141336	1926.774059	20.380544
65.203977	1922.415049	20.385562
65.434267	1918.051329	20.390579
65.320003	1921.557481	20.395597
65.652389	1916.017237	20.400615
65.685876	1923.773453	20.405632
65.585974	1913.532961	20.410650
65.624623	1916.549055	20.415667
65.618388	1919.754801	20.420685
65.942316	1910.385141	20.425703
65.773292	1920.410755	20.430720
66.006689	1916.890568	20.435738
65.986382	1914.288692	20.440755
65.439714	1907.103832	20.445773
65.773335	1905.859044	20.450791
65.636290	1916.753472	20.455808
66.117564	1898.945988	20.460826
65.882120	1913.429649	20.465843
65.792422	1919.171347	20.470861
66.202250	1915.903842	20.475879
65.890663	1929.848253	20.480896
66.210719	1931.895211	20.485914
66.229895	1937.289966	20.490931
66.331327	1937.660922	20.495949
66.437053	1946.322026	20.500967
66.321871	1947.518853	20.505984
66.446121	1955.856072	20.511002
66.457865	1970.662210	20.516019
66.449726	1979.217994	20.521037
66.960860	1972.892506	20.526055
67.000182	1979.205968	20.531072
66.718737	1975.838666	20.536090
66.892865	1977.039700	20.541107
67.048933	1987.110268	20.546125
67.644161	1995.176536	20.551143
67.645802	2001.244301	20.556160
67.879795	1985.727424	20.561178
67.559018	1975.981492	20.566195
67.384818	1978.434508	20.571213
67.785343	1973.239710	20.576231
67.582366	1989.081460	20.581248
67.895607	1987.279850	20.586266
67.956839	2002.321189	20.591283
67.997650	1987.882881	20.596301
68.480717	1990.800587	20.601319
67.905442	1985.635542	20.606336
68.123849	1982.019404	20.611354
67.935425	1986.909244	20.616371
68.132074	1993.448550	20.621389
68.315851	1989.898502	20.626407
67.996301	2001.103704	20.631424
68.125415	1996.526407	20.636442
68.318058	1999.270178	20.641459
68.439907	1997.069600	20.646477
68.267215	1993.535494	20.651495
68.189414	1997.895613	20.656512
68.467969	2012.275378	20.661530
68.718434	2022.359234	20.666547
68.543983	2031.970459	20.671565
68.903263	2014.055646	20.676583
68.830518	2026.786077	20.681600
68.694120	2024.981439	20.686618
68.852090	2029.705927	20.691635
68.765124	2033.772539	20.696653
69.510667	2040.988919	20.701671
69.451903	2052.880188	20.706688
69.425503	2041.012969	20.711706
69.650895	2049.013175	20.716723
69.554265	2043.675812	20.721741
69.820088	2044.674229	20.726759
69.714543	2044.211349	20.731776
69.799096	2044.266422	20.736794
70.223024	2043.081163	20.741811
69.824835	2031.624859	20.746829
69.870283	2024.341580	20.751847
69.896457	2038.863878	20.756864
69.924947	2041.860380	20.761882
70.257745	2033.247522	20.766899
69.875904	2050.660408	20.771917
70.239628	2043.897444	20.776935
70.063089	2047.421422	20.781952
69.891782	2042.402747	20.786970
70.162468	2052.063349	20.791987
70.118833	2065.077071	20.797005
70.133833	2074.333239	20.802023
70.323074	2074.222161	20.807040
70.689231	2071.789104	20.812058
70.872664	2074.930026	20.817075
70.694847	2076.073923	20.822093
70.576335	2071.828712	20.827111
70.829498	2081.530672	20.832128
71.130871	2088.473372	20.837146
71.061512	2084.356403	20.842163
71.432780	2099.461673	20.847181
71.790256	2087.991009	20.852199
71.373865	2093.007698	20.857216
71.414821	2090.064857	20.862234
71.703601	2083.412939	20.867251
71.621859	2088.810471	20.872269
72.077295	2086.135843	20.877287
71.947509	2090.340664	20.882304
71.762479	2086.379798	20.887322
71.746894	2085.870319	20.892339
71.640233	2090.180005	20.897357
71.970896	2091.590498	20.902375
71.609984	2089.617136	20.907392
71.635099	2085.397000	20.912410
71.834945	2091.416676	20.917427
71.717894	2105.304271	20.922445
72.014838	2114.028588	20.927463
72.283555	2122.362530	20.932480
72.054775	2119.951973	20.937498
72.519706	2112.143157	20.942515
72.308747	2124.039090	20.947533
72.546690	2131.526826	20.952551
72.429650	2145.395578	20.957568
72.253477	2143.428146	20.962586
72.618267	2139.374865	20.967603
72.678237	2148.317915	20.972621
72.805193	2138.384053	20.977639
73.056903	2150.909460	20.982656
72.892856	2166.329073	20.987674
73.208259	2174.219026	20.992691
73.255533	2172.802774	20.997709
73.676649	2167.264020	21.002727
73.345292	2174.143261	21.007744
73.481278	2176.424131	21.012762
73.780057	2176.209842	21.017779
73.442740	2171.772949	21.022797
73.687525	2172.596169	21.027815
73.638634	2169.526835	21.032832
73.653928	2178.954505	21.037850
73.714810	2171.717462	21.042867
73.810377	2181.599585	21.047885
74.204003	2180.721210	21.052903
74.432363	2195.952417	21.057920
74.308178	2196.598493	21.062938
74.482271	2194.784437	21.067955
74.042810	2193.433218	21.072973
74.427219	2192.956702	21.077991
74.328229	2203.521187	21.083008
74.196880	2194.058762	21.088026
74.383335	2198.792920	21.093043
74.521744	2208.503826	21.098061
74.792645	2216.002869	21.103079
74.768245	2223.916360	21.108096
74.866836	2226.136338	21.113114
75.172895	2229.691953	21.118131
75.062546	2230.337397	21.123149
75.126759	2219.287830	21.128167
75.124872	2227.619362	21.133184
75.402095	2222.459087	21.138202
75.437567	2215.495886	21.143219
75.554134	2218.841011	21.148237
75.795839	2211.389470	21.153255
75.829409	2215.322849	21.158272
75.562812	2216.559577	21.163290
75.725035	2206.220441	21.168307
75.927101	2210.119870	21.173325
76.130216	2205.029629	21.178343
76.185487	2208.762891	21.183360
76.071629	2205.475003	21.188378
76.363523	2202.134996	21.193395
75.976087	2208.268827	21.198413
76.199752	2213.354183	21.203431
76.609729	2222.239103	21.208448
76.175292	2236.079108	21.213466
76.652668	2231.631842	21.218483
76.709154	2240.307266	21.223501
76.591517	2243.360938	21.228519
76.573228	2238.932144	21.233536
76.601292	2242.576933	21.238554
76.799060	2230.175880	21.243571
76.631589	2241.529283	21.248589
76.757665	2235.400390	21.253607
76.615707	2247.558376	21.258624
76.665504	2268.216728	21.263642
76.930891	2262.496677	21.268659
76.941923	2278.999987	21.273677
76.937219	2270.019182	21.278695
77.327746	2274.467530	21.283712
77.512198	2270.527928	21.288730
77.585505	2277.764316	21.293747
77.494979	2294.614222	21.298765
77.841476	2299.185232	21.303783
77.940482	2291.529072	21.308800
78.080606	2302.962476	21.313818
78.075437	2292.836404	21.318835
78.138024	2287.335115	21.323853
78.175561	2284.027786	21.328871
78.478914	2282.447186	21.333888
78.354204	2286.349189	21.338906
78.760922	2283.534411	21.343923
78.360078	2284.076723	21.348941
78.223682	2280.406179	21.353959
78.427580	2278.451275	21.358976
78.247102	2286.694113	21.363994
78.688918	2284.344926	21.369011
78.307134	2305.951602	21.374029
78.809169	2312.863985	21.379047
79.110464	2311.938184	21.384064
78.908226	2318.003196	21.389082
79.449044	2314.868109	21.394099
79.155457	2315.675716	21.399117
79.454020	2304.709067	21.404135
79.595746	2306.317263	21.409152
79.309600	2312.499488	21.414170
79.415181	2304.747877	21.419187
79.560775	2302.964312	21.424205
79.270239	2307.781653	21.429223
79.618924	2320.758211	21.434240
79.658590	2329.023390	21.439258
79.979201	2335.211127	21.444275
79.805893	2327.655798	21.449293
79.925187	2332.423523	21.454311
80.487925	2327.528399	21.459328
80.258343	2331.860117	21.464346
80.413802	2330.545379	21.469363
80.366206	2325.508450	21.474381
80.180462	2326.313020	21.479399
80.007892	2328.737514	21.484416
80.160106	2342.819169	21.489434
80.386659	2343.539899	21.494451
80.357316	2358.941379	21.499469
80.560617	2360.363558	21.504487
81.051091	2357.058712	21.509504
80.571517	2362.191762	21.514522
81.217281	2369.004162	21.519539
81.189434	2390.155699	21.524557
81.470039	2382.972402	21.529575
81.318534	2385.541433	21.534592
81.120718	2387.368977	21.539610
81.504203	2379.690218	21.544627
81.526627	2393.114544	21.549645
81.424849	2388.164111	21.554663
81.477248	2378.986915	21.559680
81.576713	2389.138371	21.564698
81.419423	2380.740338	21.569715
81.704996	2390.694564	21.574733
81.658134	2400.576736	21.579751
81.677555	2409.303796	21.584768
81.812278	2420.911213	21.589786
81.846623	2414.424010	21.594803
81.976909	2428.438447	21.599821
81.950602	2443.557131	21.604839
82.571578	2449.090523	21.609856
82.303818	2452.686569	21.614874
82.698905	2444.697565	21.619891
82.631392	2445.174140	21.624909
82.679705	2447.121342	21.629927
82.748280	2458.448283	21.634944
83.026794	2470.469391	21.639962
83.399186	2459.875518	21.644979
83.563171	2460.445758	21.649997
83.320495	2466.110589	21.655015
83.470433	2463.917262	21.660032
83.582820	2465.590726	21.665050
83.699918	2462.592403	21.670067
83.881309	2471.936351	21.675085
83.775361	2471.452281	21.680103
83.478707	2465.176739	21.685120
83.590270	2468.098724	21.690138
83.494781	2456.084073	21.695155
83.636866	2468.254370	21.700173
83.429479	2469.164662	21.705191
84.133186	2467.130816	21.710208
84.075431	2484.269128	21.715226
84.122132	2488.658310	21.720243
84.015136	2485.445567	21.725261
83.925528	2487.333745	21.730279
84.025550	2489.860323	21.735296
83.875171	2511.682910	21.740314
84.485724	2508.359670	21.745331
84.781549	2512.039703	21.750349
84.684223	2521.304627	21.755367
85.100729	2503.689242	21.760384
84.599471	2516.375156	21.765402
85.069705	2525.876817	21.770419
85.418515	2534.372070	21.775437
85.486533	2532.980009	21.780455
85.637389	2533.097669	21.785472
85.517944	2532.711719	21.790490
86.079369	2530.457484	21.795507
85.758378	2513.570124	21.800525
85.656711	2513.380360	21.805543
85.778248	2494.408663	21.810560
85.531445	2513.104017	21.815578
85.717973	2525.769149	21.820595
85.787448	2533.267439	21.825613
86.034095	2533.155071	21.830631
85.923910	2528.604756	21.835648
85.799041	2546.919642	21.840666
86.218428	2547.759093	21.845683
86.346088	2563.909018	21.850701
86.315844	2568.341173	21.855719
86.205905	2563.417940	21.860736
86.423680	2576.837242	21.865754
86.470129	2566.194580	21.870771
86.759392	2574.275354	21.875789
86.651474	2589.105132	21.880807
87.209995	2591.874056	21.885824
86.991174	2597.766405	21.890842
87.244407	2608.642376	21.895859
87.318292	2595.894982	21.900877
86.549474	2605.141177	21.905895
87.089477	2595.270148	21.910912
87.040765	2620.286968	21.915930
87.358056	2630.915960	21.920947
87.262704	2634.103821	21.925965
87.676984	2643.304544	21.930983
87.751061	2637.050046	21.936000
87.881646	2645.069633	21.941018
88.196439	2649.003909	21.946035
88.491654	2646.839307	21.951053
88.349171	2649.291308	21.956071
88.423109	2643.247651	21.961088
88.747383	2649.467190	21.966106
89.050347	2646.045082	21.971123
88.924900	2642.417539	21.976141
88.578112	2646.722413	21.981159
89.114669	2629.134933	21.986176
89.219185	2645.824343	21.991194
89.187915	2630.846245	21.996211
89.459834	2621.434085	22.001229
89.114257	2618.352969	22.006247
89.336596	2607.598057	22.011264
89.350864	2600.084258	22.016282
89.341584	2606.051753	22.021299
89.598828	2621.956885	22.026317
89.573820	2628.322578	22.031335
89.752712	2622.967812	22.036352
89.601901	2634.952895	22.041370
89.578905	2629.635827	22.046387
90.057767	2624.242665	22.051405
89.809528	2625.986241	22.056423
89.896571	2630.302954	22.061440
89.893246	2626.629981	22.066458
89.943896	2626.273543	22.071475
89.794486	2629.969542	22.076493
89.672775	2648.428006	22.081511
90.242565	2660.657696	22.086528
90.081058	2666.032760	22.091546
90.071182	2668.587121	22.096563
90.203114	2678.886997	22.101581
90.535616	2697.928369	22.106599
90.434572	2694.938825	22.111616
90.698796	2704.587519	22.116634
90.770121	2716.071550	22.121651
90.818806	2718.692887	22.126669
91.103557	2724.990346	22.131687
91.415598	2713.372259	22.136704
91.474041	2722.175094	22.141722
90.963049	2719.975421	22.146739
91.583825	2733.892269	22.151757
91.578776	2746.398561	22.156775
91.880588	2741.647963	22.161792
92.158488	2740.447395	22.166810
92.324926	2739.167057	22.171827
92.571359	2743.095741	22.176845
92.332921	2738.615371	22.181863
92.589814	2737.795745	22.186880
92.537361	2731.477999	22.191898
92.499726	2737.241606	22.196915
92.714889	2739.834039	22.201933
92.499884	2738.697912	22.206951
92.431408	2736.308887	22.211968
92.330110	2738.018817	22.216986
92.552847	2740.851544	22.222003
92.863270	2748.957361	22.227021
92.563363	2774.713046	22.232039
93.158431	2771.477964	22.237056
93.030623	2777.586360	22.242074
93.029188	2779.067189	22.247091
93.480119	2783.945015	22.252109
93.467415	2808.050190	22.257127
93.549064	2800.192790	22.262144
93.564207	2799.989114	22.267162
93.520555	2798.835884	22.272179
93.519862	2799.808419	22.277197
93.632284	2811.923947	22.282215
93.951994	2822.612480	22.287232
94.226432	2821.730266	22.292250
94.361521	2827.869132	22.297267
94.659040	2830.866949	22.302285
94.552614	2824.925924	22.307303
94.795048	2834.919586	22.312320
94.439599	2834.443038	22.317338
94.254154	2829.829897	22.322355
94.631504	2828.419160	22.327373
94.755780	2828.743232	22.332391
94.726501	2825.544768	22.337408
94.839530	2840.443405	22.342426
94.778994	2855.620677	22.347443
95.119803	2859.627956	22.352461
94.726990	2867.045163	22.357479
94.959105	2857.525134	22.362496
95.206373	2878.078911	22.367514
95.425382	2882.250363	22.372531
95.956068	2893.334033	22.377549
95.676149	2895.578286	22.382567
96.237111	2887.305358	22.387584
96.261524	2884.156531	22.392602
95.985061	2894.112621	22.397619
96.327054	2887.697296	22.402637
95.997005	2883.262169	22.407655
96.030356	2885.686169	22.412672
96.629633	2896.446601	22.417690
96.420151	2894.950078	22.422707
96.799050	2900.451450	22.427725
96.472482	2902.455346	22.432743
96.821704	2893.722157	22.437760
97.373049	2886.462405	22.442778
97.166738	2882.008333	22.447795
97.397135	2873.864431	22.452813
97.449867	2885.773995	22.457831
97.719501	2879.230187	22.462848
97.741979	2887.029575	22.467866
97.689529	2883.171641	22.472883
97.687356	2879.603047	22.477901
97.603594	2878.171437	22.482919
97.738176	2873.366439	22.487936
97.935663	2885.486557	22.492954
97.909580	2905.813353	22.497971
98.245208	2901.647306	22.502989
98.118060	2912.300176	22.508007
98.293655	2907.022925	22.513024
98.595002	2911.634372	22.518042
98.601983	2910.229195	22.523059
98.705191	2907.946496	22.528077
98.481304	2912.236568	22.533095
98.440856	2913.009345	22.538112
98.452709	2914.090806	22.543130
98.440557	2924.408324	22.548147
98.857529	2930.199420	22.553165
98.457131	2936.759626	22.558183
99.233600	2957.802604	22.563200
99.288828	2967.165414	22.568218
99.364912	2975.145887	22.573235
99.749808	2966.639819	22.578253
99.626938	2971.424343	22.583271
99.691137	2969.662332	22.588288
100.095695	2967.134118	22.593306
99.784493	2969.279531	22.598323
99.969041	2966.475669	22.603341
100.206554	2970.990327	22.608359
100.094998	2965.415861	22.613376
100.042867	2968.471822	22.618394
100.379346	2989.543314	22.623411
100.750380	2990.945103	22.628429
100.663690	2990.862289	22.633447
100.384579	2987.551015	22.638464
100.678369	2985.734297	22.643482
100.773805	2992.761405	22.648499
100.575254	2991.959325	22.653517
100.706905	3000.234603	22.658535
100.763842	3020.576639	22.663552
100.871131	3015.812133	22.668570
100.744997	3019.991462	22.673587
101.474796	3037.147222	22.678605
101.086720	3053.393300	22.683623
101.002331	3052.907346	22.688640
101.773488	3048.103049	22.693658
102.021423	3060.883934	22.698675
102.335295	3071.814301	22.703693
102.334940	3074.124134	22.708711
102.431193	3073.133440	22.713728
103.369165	3063.504656	22.718746
102.814411	3045.520369	22.723763
102.898978	3027.700051	22.728781
102.979763	3022.393824	22.733799
102.818281	3032.641618	22.738816
103.311310	3028.054745	22.743834
102.990172	3033.526196	22.748851
102.896945	3027.310798	22.753869
103.071323	3028.205084	22.758887
103.280441	3026.415238	22.763904
102.806465	3027.880976	22.768922
102.961729	3046.018081	22.773939
103.505555	3047.103616	22.778957
103.440563	3057.310867	22.783975
103.261305	3059.339279	22.788992
103.616261	3071.546148	22.794010
103.570836	3081.091855	22.799027
103.459924	3093.037909	22.804045
103.772795	3091.305457	22.809063
104.215486	3107.489921	22.814080
104.252679	3111.497698	22.819098
104.203288	3122.117081	22.824115
104.573250	3120.226055	22.829133
104.618135	3119.977511	22.834151
104.582647	3124.951112	22.839168
104.969046	3119.740865	22.844186
104.817219	3120.905868	22.849203
105.114089	3123.071553	22.854221
105.252120	3139.572101	22.859239
105.024026	3144.669248	22.864256
105.317041	3140.959120	22.869274
105.192787	3150.299534	22.874291
105.338155	3139.649336	22.879309
105.245708	3142.116252	22.884327
105.123993	3149.461264	22.889344
105.698784	3158.531306	22.894362
105.789439	3190.076704	22.899379
105.878934	3174.658710	22.904397
105.650909	3183.350954	22.909415
105.986010	3176.930310	22.914432
106.256454	3192.003232	22.919450
106.581758	3203.512440	22.924467
106.604351	3196.338426	22.929485
106.675014	3208.222579	22.934503
106.084807	3208.164200	22.939520
106.617770	3206.611401	22.944538
106.614268	3232.191607	22.949555
106.902932	3230.762723	22.954573
106.976579	3230.724354	22.959591
107.160453	3233.272305	22.964608
107.199880	3236.978463	22.969626
107.327727	3252.878168	22.974643
107.639170	3256.406434	22.979661
107.684381	3261.834499	22.984679
107.459217	3265.570269	22.989696
107.784377	3254.483034	22.994714
107.628366	3271.850335	22.999731
108.100327	3286.260305	23.004749
108.614087	3285.445319	23.009767
108.312576	3284.595132	23.014784
108.860505	3272.714003	23.019802
108.934187	3273.240463	23.024819
109.061736	3270.474740	23.029837
109.478422	3274.900349	23.034855
109.421200	3274.564243	23.039872
109.574059	3266.137485	23.044890
109.192563	3274.229633	23.049907
109.627761	3267.875590	23.054925
109.226783	3275.265194	23.059943
109.403505	3272.002317	23.064960
109.442334	3271.066394	23.069978
109.578232	3277.236788	23.074995
109.680738	3263.694426	23.080013
109.682959	3264.569766	23.085031
110.216322	3287.717016	23.090048
110.011660	3288.135245	23.095066
110.287238	3294.208639	23.100083
110.156927	3290.519562	23.105101
110.283248	3291.466369	23.110119
109.911393	3292.965408	23.115136
110.544172	3290.680808	23.120154
110.530655	3314.167041	23.125171
110.615805	3310.887289	23.130189
110.706458	3319.005655	23.135207
110.690286	3328.013488	23.140224
110.906874	3320.474140	23.145242
111.079767	3329.800327	23.150259
111.113617	3343.192233	23.155277
111.447065	3344.847857	23.160295
111.253991	3354.842093	23.165312
111.675287	3339.957097	23.170330
111.524774	3344.053869	23.175347
111.405217	3353.671362	23.180365
111.903213	3368.742008	23.185383
112.050910	3373.691990	23.190400
112.142110	3379.132432	23.195418
112.179408	3382.366956	23.200435
112.299441	3379.275938	23.205453
112.797344	3388.326132	23.210471
112.636155	3401.812914	23.215488
112.828871	3396.527252	23.220506
112.744815	3400.459253	23.225523
112.610605	3404.522762	23.230541
113.237683	3397.326996	23.235559
112.920956	3407.180501	23.240576
113.306687	3419.669895	23.245594
113.385189	3430.782813	23.250611
113.363828	3432.851393	23.255629
113.763562	3435.227289	23.260647
113.613996	3432.335013	23.265664
113.747351	3426.947097	23.270682
113.963390	3443.682568	23.275699
113.860332	3451.734346	23.280717
114.264612	3450.309821	23.285735
114.181660	3450.716513	23.290752
114.195122	3449.362173	23.295770
114.240394	3463.952066	23.300787
114.847484	3474.716404	23.305805
115.053276	3481.077919	23.310823
114.980374	3493.395060	23.315840
115.096601	3491.140090	23.320858
115.027261	3492.509094	23.325875
115.314587	3492.516109	23.330893
115.415870	3487.001121	23.335911
115.278292	3494.930983	23.340928
115.351678	3516.881438	23.345946
115.437677	3517.870877	23.350963
115.717609	3513.047216	23.355981
115.853431	3518.110063	23.360999
116.017436	3522.410835	23.366016
116.068565	3537.995032	23.371034
116.088317	3552.397129	23.376051
116.096211	3552.694149	23.381069
116.568106	3553.681060	23.386087
116.552145	3548.183171	23.391104
116.554855	3552.017988	23.396122
116.732078	3572.063905	23.401139
117.021774	3578.971422	23.406157
117.084858	3581.377423	23.411175
117.256487	3584.613386	23.416192
117.138523	3571.456763	23.421210
117.446077	3572.895482	23.426227
117.150601	3569.655125	23.431245
117.586903	3580.785840	23.436263
117.483896	3591.839713	23.441280
118.221971	3597.830046	23.446298
118.167705	3611.513951	23.451315
118.106035	3602.492639	23.456333
118.298174	3599.941551	23.461351
118.205012	3599.162752	23.466368
118.537715	3587.170940	23.471386
118.397823	3593.050311	23.476403
118.388517	3601.522264	23.481421
119.067707	3607.925566	23.486439
118.698138	3623.809798	23.491456
119.166985	3615.859543	23.496474
119.088773	3626.967703	23.501491
119.339375	3620.952904	23.506509
119.745134	3609.910768	23.511527
119.184315	3613.963688	23.516544
119.276238	3620.783183	23.521562
119.897360	3638.078922	23.526579
119.675401	3650.496271	23.531597
119.633655	3648.291641	23.536615
119.620812	3659.038536	23.541632
119.764444	3660.291780	23.546650
119.803731	3669.151733	23.551667
120.115727	3681.755379	23.556685
120.533316	3666.360865	23.561703
120.905557	3692.538851	23.566720
121.233152	3696.930021	23.571738
121.310462	3703.689736	23.576755
121.534006	3709.690570	23.581773
121.641709	3696.304324	23.586791
122.014115	3689.548671	23.591808
121.946913	3664.234864	23.596826
121.778285	3651.352939	23.601843
122.038748	3652.611154	23.606861
122.081049	3636.549603	23.611879
121.831354	3646.578239	23.616896
122.146825	3663.792940	23.621914
122.361662	3672.502178	23.626931
122.265725	3674.688887	23.631949
122.582323	3676.011317	23.636967
122.619136	3679.984696	23.641984
122.513538	3678.923090	23.647002
122.397644	3678.658479	23.652019
122.292189	3686.016112	23.657037
122.855606	3686.526648	23.662055
122.779284	3697.850903	23.667072
122.960952	3702.541475	23.672090
122.756780	3703.421429	23.677107
122.614628	3726.287669	23.682125
123.011562	3728.631021	23.687143
123.481453	3724.672270	23.692160
124.721661	3718.077966	23.697178
124.777660	3710.253279	23.702195
124.820826	3702.751616	23.707213
124.705464	3699.827871	23.712231
124.873336	3705.688109	23.717248
125.000373	3699.403475	23.722266
125.011692	3692.661341	23.727283
124.684604	3699.051277	23.732301
125.117615	3695.468163	23.737319
125.192090	3694.807382	23.742336
125.109259	3690.087922	23.747354
125.258596	3695.041685	23.752371
124.868172	3690.688310	23.757389
125.530036	3685.149946	23.762407
125.156051	3690.429455	23.767424
124.890852	3707.903578	23.772442
125.337561	3716.257257	23.777459
125.410312	3732.395198	23.782477
125.565723	3735.548818	23.787495
125.750191	3754.505033	23.792512
125.889672	3757.739868	23.797530
126.174690	3764.980209	23.802547
125.964642	3786.475917	23.807565
126.019017	3787.896812	23.812583
126.255810	3792.956242	23.817600
126.256797	3811.121252	23.822618
126.428205	3823.962997	23.827635
126.759974	3827.602236	23.832653
127.123452	3839.944490	23.837671
127.247923	3852.971540	23.842688
127.733398	3850.095143	23.847706
127.658077	3853.732429	23.852723
127.734755	3855.286662	23.857741
128.159894	3846.375602	23.862759
128.166387	3855.580754	23.867776
128.624446	3870.810124	23.872794
128.642803	3883.629122	23.877811
128.473872	3882.913525	23.882829
128.562577	3879.198817	23.887847
128.203917	3883.450080	23.892864
128.471119	3874.515410	23.897882
128.626882	3884.543280	23.902899
128.388106	3906.382814	23.907917
128.941539	3906.638485	23.912935
128.975840	3906.402630	23.917952
128.767650	3930.010571	23.922970
129.207725	3939.800401	23.927987
129.179201	3940.997728	23.933005
129.697575	3954.285399	23.938023
130.010761	3968.205277	23.943040
130.334034	3962.524908	23.948058
130.494395	3957.570693	23.953075
130.454230	3965.919542	23.958093
130.902415	3945.541529	23.963111
130.892075	3957.429764	23.968128
130.781770	3953.004897	23.973146
130.896756	3950.183622	23.978163
131.012104	3951.130650	23.983181
130.985859	3954.426569	23.988199
130.971767	3955.345460	23.993216
131.017504	3951.352007	23.998234
131.336817	3961.545810	24.003251
130.899196	3977.479821	24.008269
131.447177	3974.908907	24.013287
131.740846	3977.695953	24.018304
131.874391	3983.766321	24.023322
132.079778	4004.351172	24.028339
132.003128	4007.529265	24.033357
132.337666	4011.929652	24.038375
132.624488	4013.990083	24.043392
132.223421	4012.159738	24.048410
132.559183	4022.724652	24.053427
132.397862	4035.760456	24.058445
132.678474	4035.511288	24.063463
132.706626	4031.640200	24.068480
132.781196	4063.533832	24.073498
132.887661	4058.205045	24.078515
133.465753	4071.706730	24.083533
133.655300	4088.537634	24.088551
133.755747	4100.347741	24.093568
133.944161	4102.858147	24.098586
134.173111	4099.465606	24.103603
134.299040	4106.593807	24.108621
134.309608	4102.223575	24.113639
134.269991	4098.020264	24.118656
134.207565	4117.273571	24.123674
134.663463	4124.088763	24.128691
134.961062	4124.017045	24.133709
135.480895	4113.538522	24.138727
135.608673	4103.677944	24.143744
135.357083	4113.456233	24.148762
135.887029	4107.396698	24.153779
135.607045	4105.295283	24.158797
135.961946	4108.464379	24.163815
136.127546	4106.684492	24.168832
135.831787	4113.062528	24.173850
136.241844	4119.022779	24.178867
136.239471	4131.793374	24.183885
136.313070	4134.936524	24.188903
136.538320	4138.389851	24.193920
136.659642	4136.462823	24.198938
136.554680	4127.634544	24.203955
136.710940	4147.410810	24.208973
137.079901	4156.421466	24.213991
136.975191	4163.250538	24.219008
136.803993	4160.401688	24.224026
137.223847	4165.092195	24.229043
137.078916	4181.045840	24.234061
137.504474	4184.496349	24.239079
137.696442	4195.818331	24.244096
137.504953	4199.654385	24.249114
137.907508	4192.930675	24.254131
137.689988	4222.019338	24.259149
137.994293	4225.984829	24.264167
138.149293	4223.614212	24.269184
138.193253	4230.953012	24.274202
138.379320	4248.133174	24.279219
138.434438	4259.539964	24.284237
138.645421	4265.492680	24.289255
138.960047	4274.796082	24.294272
138.970272	4287.601780	24.299290
139.766293	4281.849847	24.304307
139.259322	4286.849450	24.309325
139.251603	4294.765329	24.314343
139.666140	4313.075863	24.319360
139.435264	4329.702654	24.324378
139.946548	4324.801721	24.329395
140.051299	4339.350742	24.334413
140.231244	4337.433222	24.339431
140.385550	4344.137685	24.344448
140.128283	4349.549081	24.349466
140.588844	4359.200608	24.354483
140.577144	4376.850665	24.359501
140.773248	4380.678464	24.364519
141.207391	4374.841796	24.369536
141.365847	4391.298796	24.374554
141.926800	4400.599193	24.379571
141.938618	4403.590183	24.384589
141.751566	4400.693463	24.389607
142.281364	4389.344600	24.394624
141.964250	4400.300256	24.399642
142.443360	4391.108842	24.404659
142.364084	4397.024497	24.409677
142.578553	4392.771148	24.414695
142.859108	4406.828030	24.419712
143.048450	4416.588925	24.424730
142.818842	4414.013683	24.429747
142.915308	4416.443609	24.434765
143.394967	4415.678855	24.439783
143.432527	4409.894392	24.444800
143.259843	4422.238445	24.449818
143.550450	4433.405630	24.454835
143.497157	4445.600855	24.459853
144.006734	4443.925792	24.464871
144.181739	4447.650762	24.469888
143.931236	4446.505207	24.474906
144.006765	4467.087808	24.479923
144.179972	4480.323209	24.484941
144.127517	4482.612461	24.489959
144.474606	4492.099644	24.494976
144.686499	4514.578648	24.499994
145.266853	4500.674162	24.505011
145.040196	4510.278800	24.510029
145.235897	4503.005742	24.515047
145.834509	4489.200633	24.520064
145.710920	4493.162042	24.525082
146.226268	4495.710864	24.530099
146.039947	4499.100087	24.535117
146.271545	4508.383834	24.540135
146.713059	4509.295416	24.545152
146.070213	4518.400747	24.550170
146.736370	4524.406874	24.555187
146.741960	4510.923667	24.560205
146.721038	4513.551702	24.565223
147.236228	4514.494809	24.570240
146.955489	4507.949137	24.575258
147.286863	4503.629126	24.580275
147.426707	4515.601649	24.585293
147.428869	4520.266820	24.590311
147.649383	4533.394024	24.595328
147.573563	4536.535907	24.600346
148.013785	4529.540121	24.605363
147.939378	4534.243468	24.610381
147.778749	4539.418449	24.615399
148.143113	4550.506303	24.620416
148.220934	4557.133369	24.625434
148.270469	4551.095182	24.630451
148.092625	4581.119960	24.635469
148.471190	4581.180095	24.640487
148.669211	4596.310854	24.645504
148.502443	4621.273581	24.650522
149.139074	4615.277869	24.655539
149.528109	4621.687766	24.660557
149.571679	4638.260917	24.665575
149.777693	4638.815895	24.670592
149.944644	4647.353182	24.675610
150.159695	4632.982055	24.680627
150.158628	4655.495229	24.685645
150.270272	4665.782427	24.690663
150.472570	4663.948632	24.695680
150.681647	4675.287138	24.700698
150.875165	4673.802486	24.705715
151.110728	4681.409141	24.710733
151.328907	4698.698788	24.715751
151.540613	4690.633973	24.720768
151.558795	4702.489937	24.725786
151.869915	4694.325873	24.730803
151.921342	4684.190705	24.735821
152.101151	4681.886081	24.740839
152.544111	4673.233677	24.745856
152.296610	4686.023379	24.750874
152.358106	4687.775236	24.755891
153.115570	4701.079754	24.760909
152.801080	4704.935548	24.765927
153.273291	4705.021666	24.770944
152.964677	4711.079437	24.775962
153.591817	4694.819636	24.780979
153.497833	4709.437687	24.785997
153.342173	4710.775720	24.791015
153.873883	4697.830781	24.796032
153.560136	4707.962394	24.801050
153.572070	4705.225855	24.806067
153.924242	4717.536823	24.811085
153.915888	4726.415236	24.816103
154.023416	4726.904098	24.821120
154.082782	4736.820465	24.826138
154.470711	4738.758669	24.831155
154.887328	4752.756425	24.836173
155.003410	4750.155903	24.841191
155.018875	4745.155295	24.846208
154.992453	4754.263978	24.851226
155.142420	4755.229929	24.856243
155.674451	4767.103936	24.861261
155.750228	4781.152915	24.866279
155.835159	4776.396917	24.871296
156.057038	4782.541649	24.876314
156.209279	4774.510659	24.881331
156.144717	4790.201170	24.886349
156.215273	4809.693808	24.891367
156.841007	4807.924659	24.896384
156.160437	4816.121969	24.901402
156.813984	4818.482024	24.906419
156.948131	4831.698793	24.911437
156.931865	4838.375604	24.916455
157.157932	4843.112965	24.921472
157.048552	4855.143595	24.926490
157.200936	4866.022376	24.931507
157.679174	4876.743787	24.936525
157.697558	4896.315665	24.941543
158.131312	4898.554998	24.946560
158.082216	4910.553245	24.951578
158.061381	4914.279662	24.956595
158.314219	4934.600976	24.961613
158.459893	4948.863985	24.966631
158.571987	4951.693546	24.971648
158.591305	4968.617112	24.976666
159.088579	4972.712543	24.981683
159.075092	4978.880721	24.986701
159.117605	4995.827370	24.991719
159.662224	4996.056154	24.996736
159.744223	4993.896108	25.001754
160.071047	5005.769981	25.006771
160.632480	5016.930623	25.011789
160.427149	5026.883093	25.016807
160.480230	5027.818091	25.021824
160.420317	5033.993694	25.026842
160.938493	5034.194438	25.031859
161.046423	5051.356524	25.036877
161.106460	5051.007974	25.041895
161.336118	5050.314525	25.046912
161.106687	5048.039688	25.051930
161.058866	5071.062123	25.056947
161.709936	5082.763986	25.061965
161.663635	5084.356053	25.066983
161.943938	5083.433444	25.072000
162.014398	5097.523697	25.077018
162.483388	5103.157887	25.082035
162.582150	5115.086306	25.087053
162.279829	5113.427324	25.092071
162.777770	5114.683215	25.097088
162.905247	5136.164832	25.102106
162.931196	5143.043545	25.107123
163.049971	5141.309555	25.112141
163.054399	5151.180671	25.117159
163.609648	5164.943501	25.122176
163.476672	5178.166190	25.127194
163.739760	5184.206173	25.132211
163.890323	5198.474938	25.137229
163.694660	5211.046755	25.142247
163.805293	5213.012713	25.147264
164.059995	5226.824305	25.152282
164.442574	5236.912922	25.157299
164.722783	5255.268077	25.162317
164.674296	5258.936833	25.167335
164.986936	5267.641655	25.172352
165.205792	5291.344968	25.177370
165.860593	5288.172229	25.182387
166.140085	5288.491285	25.187405
166.194397	5299.288461	25.192423
166.796165	5290.712665	25.197440
166.594073	5285.872446	25.202458
166.567066	5284.142012	25.207475
166.597905	5302.121561	25.212493
166.746840	5318.862784	25.217511
167.131578	5313.351493	25.222528
167.360435	5328.078399	25.227546
167.132175	5327.716012	25.232563
167.475708	5341.449818	25.237581
167.345710	5366.197864	25.242599
167.494965	5354.690215	25.247616
167.766659	5364.978347	25.252634
167.817927	5381.622701	25.257651
168.284221	5375.329692	25.262669
168.374521	5391.448552	25.267687
168.469301	5404.483280	25.272704
168.798992	5418.216218	25.277722
168.760237	5412.690584	25.282739
169.313502	5410.368795	25.287757
169.241067	5436.745881	25.292775
169.333656	5429.036405	25.297792
169.825059	5426.047049	25.302810
169.878572	5414.609694	25.307827
170.297701	5423.025400	25.312845
170.540993	5439.953135	25.317863
170.576132	5445.249856	25.322880
170.660120	5459.829255	25.327898
170.768249	5447.087318	25.332915
171.246923	5449.816830	25.337933
170.853681	5452.613756	25.342951
171.217370	5444.460572	25.347968
171.076910	5449.268367	25.352986
171.244842	5463.765937	25.358003
171.475671	5474.280963	25.363021
171.503389	5478.482087	25.368039
171.481331	5485.293867	25.373056
171.632797	5500.059247	25.378074
171.895893	5504.261404	25.383091
172.648279	5498.279151	25.388109
172.666627	5521.613535	25.393127
172.926802	5524.074980	25.398144
173.018848	5517.809320	25.403162
173.204345	5524.206431	25.408179
173.106507	5529.219891	25.413197
173.410671	5543.392902	25.418215
173.653399	5548.226184	25.423232
173.813996	5558.415718	25.428250
173.545761	5561.222632	25.433267
173.903940	5571.918059	25.438285
174.316762	5583.738561	25.443303
174.366501	5589.128996	25.448320
174.673691	5598.721608	25.453338
174.807316	5614.608779	25.458355
174.791367	5615.249540	25.463373
174.860888	5623.987039	25.468391
175.368403	5630.551588	25.473408
175.546001	5645.836959	25.478426
175.400734	5649.900481	25.483443
175.822336	5665.085599	25.488461
175.702194	5681.676577	25.493479
176.306821	5678.087671	25.498496
176.382264	5684.024806	25.503514
176.563665	5701.570909	25.508531
177.265305	5694.769736	25.513549
177.394825	5705.774737	25.518567
177.571246	5696.932917	25.523584
177.580880	5688.427696	25.528602
177.603827	5689.986757	25.533619
178.021666	5698.543666	25.538637
178.206997	5718.776896	25.543655
178.018120	5722.271447	25.548672
178.509749	5717.752443	25.553690
178.496882	5714.339870	25.558707
178.714883	5714.693132	25.563725
178.700677	5733.671764	25.568743
178.975313	5738.921753	25.573760
179.519342	5742.635429	25.578778
179.001996	5743.381311	25.583795
179.321934	5749.101674	25.588813
179.496703	5777.320429	25.593831
179.472025	5780.695185	25.598848
179.842604	5783.734689	25.603866
180.029880	5798.558390	25.608883
180.240427	5806.506371	25.613901
180.218601	5814.199496	25.618919
180.351746	5815.397951	25.623936
180.722505	5827.423633	25.628954
180.862519	5833.024006	25.633971
181.404029	5828.223993	25.638989
181.771216	5833.943150	25.644007
181.642228	5833.077097	25.649024
181.761185	5840.964164	25.654042
181.996772	5859.726100	25.659059
182.324895	5853.056006	25.664077
182.374981	5856.073447	25.669095
182.569969	5851.812564	25.674112
182.543916	5856.654179	25.679130
182.391409	5882.165162	25.684148
182.933266	5875.615986	25.689165
182.844006	5887.984935	25.694183
183.062629	5912.706636	25.699200
183.472435	5913.713070	25.704218
183.117694	5924.146312	25.709236
183.391745	5935.233089	25.714253
183.248354	5954.334884	25.719271
183.949836	5968.190030	25.724288
184.402280	5979.263349	25.729306
184.135280	5991.890472	25.734324
184.703209	6004.471048	25.739341
185.044837	6022.394840	25.744359
184.982102	6016.170170	25.749376
185.162608	6034.474522	25.754394
185.410084	6044.487667	25.759412
185.966923	6036.237277	25.764429
186.049212	6041.066401	25.769447
186.414273	6061.132964	25.774464
186.568798	6058.330954	25.779482
186.469472	6069.287732	25.784500
186.579188	6064.030884	25.789517
186.840962	6080.771502	25.794535
186.927656	6093.735737	25.799552
187.220710	6095.788396	25.804570
187.098910	6110.557822	25.809588
187.861283	6114.257244	25.814605
187.923286	6125.140347	25.819623
188.285941	6129.729669	25.824640
188.657528	6124.491637	25.829658
188.470929	6120.192371	25.834676
188.670208	6129.807254	25.839693
188.747435	6145.393188	25.844711
188.828266	6149.348411	25.849728
188.815756	6148.477145	25.854746
188.796832	6175.221541	25.859764
189.405143	6180.951178	25.864781
189.761412	6190.286925	25.869799
189.760924	6202.055792	25.874816
190.216592	6211.976847	25.879834
190.387233	6217.470981	25.884852
190.506824	6210.217096	25.889869
190.517343	6215.799703	25.894887
190.758764	6222.660303	25.899904
191.057022	6231.033583	25.904922
190.861487	6242.737583	25.909940
191.440071	6236.131252	25.914957
191.381277	6245.529272	25.919975
191.062760	6260.906172	25.924992
191.732991	6265.398505	25.930010
191.609395	6270.542215	25.935028
191.723448	6287.724427	25.940045
191.929971	6298.096777	25.945063
192.491992	6312.890362	25.950080
192.644216	6315.437608	25.955098
192.538416	6328.790749	25.960116
192.885499	6339.714325	25.965133
193.123819	6352.515343	25.970151
193.191623	6360.168102	25.975168
193.953633	6373.725998	25.980186
193.972780	6379.812444	25.985204
194.321515	6381.451830	25.990221
194.642594	6391.669858	25.995239
194.589682	6409.432768	26.000256
194.889133	6414.160511	26.005274
194.599280	6415.099124	26.010292
195.078724	6411.855761	26.015309
195.588367	6433.826763	26.020327
195.270006	6437.228029	26.025344
195.622152	6444.194615	26.030362
195.659023	6464.775137	26.035380
195.493848	6475.517672	26.040397
195.939455	6488.988418	26.045415
196.265548	6500.256165	26.050432
196.372914	6509.063690	26.055450
196.444295	6532.280259	26.060468
197.173127	6529.487322	26.065485
197.342621	6538.583176	26.070503
197.278834	6558.627506	26.075520
197.693841	6561.077035	26.080538
197.821927	6562.560412	26.085556
198.059298	6584.836279	26.090573
198.228776	6600.129436	26.095591
198.190818	6607.576109	26.100608
198.524646	6613.920145	26.105626
198.316298	6637.615818	26.110644
198.913521	6634.909153	26.115661
199.330699	6653.208798	26.120679
199.293628	6666.715737	26.125696
199.682412	6662.622018	26.130714
199.658055	6674.762525	26.135732
199.925212	6684.003418	26.140749
199.886107	6691.335434	26.145767
200.202787	6711.326397	26.150784
200.413693	6714.460797	26.155802
200.662356	6724.570997	26.160820
201.218525	6739.031527	26.165837
201.431626	6746.866299	26.170855
201.445745	6756.253016	26.175872
201.426763	6753.461226	26.180890
201.448292	6763.346424	26.185908
201.875299	6770.468832	26.190925
202.130607	6784.092934	26.195943
202.299045	6785.542361	26.200960
202.649749	6789.784428	26.205978
202.523291	6806.037738	26.210996
202.876681	6805.595172	26.216013
203.129210	6817.878142	26.221031
203.093006	6840.561537	26.226048
203.484375	6833.801453	26.231066
203.536389	6839.465022	26.236084
204.052301	6854.458497	26.241101
204.445796	6856.823377	26.246119
204.356513	6866.121993	26.251136
204.574549	6875.743026	26.256154
204.517589	6892.846185	26.261172
204.526064	6893.505140	26.266189
205.111981	6913.524272	26.271207
205.238075	6916.185949	26.276224
205.923989	6926.649132	26.281242
205.911923	6934.978646	26.286260
206.578218	6938.760485	26.291277
206.545400	6931.626545	26.296295
206.601237	6944.460313	26.301312
206.860588	6945.183143	26.306330
206.943612	6969.902253	26.311348
207.117522	6959.366735	26.316365
207.732174	6960.553836	26.321383
207.658731	6963.128514	26.326400
208.055634	6975.158832	26.331418
207.958898	6996.363347	26.336436
208.167106	6997.431903	26.341453
208.754199	6988.538804	26.346471
208.559423	6996.585876	26.351488
208.651008	7005.249852	26.356506
209.196799	7004.626316	26.361524
209.748643	7001.006966	26.366541
209.820623	6994.938243	26.371559
210.203527	7012.759869	26.376576
210.327852	7023.045896	26.381594
210.364595	7032.101052	26.386612
210.898659	7028.888198	26.391629
211.129444	7021.679144	26.396647
211.233575	7016.891831	26.401664
211.369392	7009.766380	26.406682
211.566899	7017.181229	26.411700
211.488191	7017.856448	26.416717
211.715712	7014.977314	26.421735
211.798064	7027.757353	26.426752
211.849758	7039.466629	26.431770
211.844179	7049.075422	26.436788
211.998908	7055.266432	26.441805
212.136678	7065.551919	26.446823
212.233033	7089.210749	26.451840
212.708085	7084.077074	26.456858
212.867779	7112.989288	26.461876
213.311103	7112.725951	26.466893
213.518511	7115.020605	26.471911
213.275595	7129.337430	26.476928
213.451753	7144.416837	26.481946
213.617927	7161.043292	26.486964
213.727085	7177.650527	26.491981
214.252352	7187.170063	26.496999
214.134241	7213.597708	26.502016
214.755227	7214.493461	26.507034
215.008199	7232.930557	26.512052
214.961079	7241.291010	26.517069
215.173457	7252.722639	26.522087
214.934661	7268.816916	26.527104
215.491473	7288.566177	26.532122
215.718618	7306.017179	26.537140
216.242428	7327.631966	26.542157
216.725082	7328.899553	26.547175
216.706715	7344.305650	26.552192
217.142380	7358.135629	26.557210
217.394767	7365.738627	26.562228
217.211535	7371.088157	26.567245
218.005016	7376.059297	26.572263
218.335862	7369.715448	26.577280
219.137807	7371.128471	26.582298
218.974974	7368.406712	26.587316
219.012243	7371.113321	26.592333
219.557729	7386.446102	26.597351
219.254797	7401.566338	26.602368
219.416165	7405.118364	26.607386
219.442290	7411.131331	26.612404
219.451970	7430.335335	26.617421
219.997726	7425.510149	26.622439
220.293281	7447.338156	26.627456
220.492910	7454.645473	26.632474
220.859073	7463.931268	26.637492
220.991048	7468.196992	26.642509
220.885046	7472.566752	26.647527
221.165240	7494.216682	26.652544
221.266333	7495.894888	26.657562
221.670918	7523.506275	26.662580
221.576317	7539.612086	26.667597
222.172789	7537.582914	26.672615
222.191368	7562.436822	26.677632
222.425680	7566.578454	26.682650
222.734819	7582.029377	26.687668
222.890446	7595.522176	26.692685
223.234290	7592.958038	26.697703
223.125540	7623.708182	26.702720
223.714785	7628.320087	26.707738
223.730893	7638.401094	26.712756
223.658729	7663.716601	26.717773
223.925103	7656.934370	26.722791
224.199020	7683.168149	26.727808
224.702412	7691.328567	26.732826
224.793201	7698.128878	26.737844
224.806903	7715.560873	26.742861
225.161224	7718.734006	26.747879
225.224535	7736.305270	26.752896
225.802070	7748.178762	26.757914
225.885743	7748.479918	26.762932
225.932218	7777.981980	26.767949
226.139213	7776.610166	26.772967
226.647297	7806.683972	26.777984
226.701788	7817.868537	26.783002
227.134804	7832.058215	26.788020
227.341245	7848.194274	26.793037
227.764254	7847.921578	26.798055
227.894052	7861.668582	26.803072
228.144218	7870.199579	26.808090
228.288345	7875.817774	26.813108
228.229255	7893.665665	26.818125
228.815388	7911.667260	26.823143
229.004573	7916.299748	26.828160
229.054237	7936.651658	26.833178
229.362706	7940.796132	26.838196
229.574119	7960.516752	26.843213
229.823446	7967.854172	26.848231
229.886436	7979.743376	26.853248
230.244634	7990.642791	26.858266
231.174966	7990.851484	26.863284
231.051700	7994.205469	26.868301
231.208807	8009.791634	26.873319
231.648037	8019.527271	26.878336
232.040406	8023.722529	26.883354
232.169636	8024.756536	26.888372
232.414002	8047.643345	26.893389
232.788197	8053.451963	26.898407
232.472294	8058.548639	26.903424
232.648600	8055.542514	26.908442
233.384801	8065.339045	26.913460
233.090282	8082.479071	26.918477
233.249556	8090.464781	26.923495
233.620340	8114.408852	26.928512
233.838750	8116.747552	26.933530
234.198880	8123.502368	26.938548
234.054964	8149.497845	26.943565
234.540680	8145.606262	26.948583
234.524172	8170.541137	26.953600
234.940920	8187.811854	26.958618
235.036329	8193.180999	26.963636
234.965910	8206.584079	26.968653
235.567187	8220.205892	26.973671
236.071224	8234.861912	26.978688
236.333231	8235.351847	26.983706
236.847390	8241.466382	26.988724
236.415109	8270.403586	26.993741
236.799277	8268.526600	26.998759
236.873725	8273.554828	27.003776
237.079957	8297.440433	27.008794
237.411018	8297.014770	27.013812
237.421414	8315.138140	27.018829
237.702848	8327.556645	27.023847
238.404638	8336.444411	27.028864
238.543146	8356.766204	27.033882
238.675212	8366.477452	27.038900
238.811124	8372.830579	27.043917
239.347513	8379.849373	27.048935
239.023181	8397.693713	27.053952
239.150405	8412.890801	27.058970
239.525833	8425.502553	27.063988
239.917260	8449.063772	27.069005
240.079017	8460.090066	27.074023
240.027050	8480.103212	27.079040
240.409980	8492.463574	27.084058
240.873720	8505.853780	27.089076
240.830039	8526.893823	27.094093
241.688071	8539.220987	27.099111
242.281978	8541.831209	27.104128
242.339314	8554.271066	27.109146
243.060544	8559.670828	27.114164
243.244841	8567.419077	27.119181
243.207632	8569.390952	27.124199
243.271160	8563.808103	27.129216
243.530595	8583.648590	27.134234
244.016288	8592.192430	27.139252
243.532920	8602.811713	27.144269
244.102831	8617.715340	27.149287
244.359020	8632.599737	27.154304
244.299038	8646.852644	27.159322
244.897425	8648.865655	27.164340
244.575063	8671.114633	27.169357
245.030532	8689.651098	27.174375
245.327034	8703.958197	27.179392
245.438155	8719.486327	27.184410
245.730769	8730.426250	27.189428
245.390827	8753.380126	27.194445
245.932874	8759.891392	27.199463
246.629115	8796.391912	27.204480
246.027540	8818.795004	27.209498
246.871411	8831.020001	27.214516
246.839918	8858.285875	27.219533
247.329997	8869.461601	27.224551
247.741596	8892.746043	27.229568
248.178912	8909.787667	27.234586
248.452151	8917.989385	27.239604
248.020410	8946.670850	27.244621
248.860803	8954.308423	27.249639
249.231303	8967.021759	27.254656
249.075009	8993.228822	27.259674
249.758292	9000.614839	27.264692
249.634759	9012.374442	27.269709
249.624697	9032.480408	27.274727
250.128256	9045.473228	27.279744
250.356952	9060.051180	27.284762
250.812167	9075.298177	27.289780
250.810285	9091.654117	27.294797
251.294246	9094.835610	27.299815
251.523507	9108.560820	27.304832
251.674343	9134.303643	27.309850
252.244533	9142.665916	27.314868
252.455693	9136.280599	27.319885
253.028764	9150.159990	27.324903
253.334087	9167.800597	27.329920
253.292772	9166.110948	27.334938
253.759677	9167.983265	27.339956
253.801110	9194.032848	27.344973
254.523441	9195.387932	27.349991
254.988871	9182.832193	27.355008
254.997406	9183.404670	27.360026
255.266797	9183.875757	27.365044
255.329204	9200.991245	27.370061
255.448288	9203.850413	27.375079
255.755629	9205.475082	27.380096
255.794294	9216.579791	27.385114
255.875925	9224.942861	27.390132
255.885159	9239.890047	27.395149
256.428802	9257.631284	27.400167
256.533673	9264.122347	27.405184
256.186020	9285.752961	27.410202
256.712404	9308.654587	27.415220
257.068025	9332.214245	27.420237
257.161746	9341.399832	27.425255
257.875629	9371.017427	27.430272
257.851159	9388.257549	27.435290
258.271422	9402.170189	27.440308
258.472259	9434.283813	27.445325
258.574523	9447.814724	27.450343
259.395129	9458.984642	27.455360
259.545473	9482.401360	27.460378
259.612207	9485.555003	27.465396
259.927692	9506.961394	27.470413
259.992625	9512.844671	27.475431
260.387613	9539.747884	27.480448
260.605873	9554.730142	27.485466
260.959806	9562.957915	27.490484
261.241441	9586.881559	27.495501
261.571124	9603.452789	27.500519
262.004855	9614.264618	27.505536
262.218046	9623.348699	27.510554
262.818393	9634.246135	27.515572
262.587254	9637.380392	27.520589
262.936208	9649.455341	27.525607
263.190339	9653.932028	27.530624
263.127210	9679.733893	27.535642
263.665761	9693.503994	27.540660
263.657542	9704.644081	27.545677
263.699642	9725.365974	27.550695
264.107151	9728.376417	27.555712
264.083996	9742.388383	27.560730
264.897021	9758.304283	27.565748
264.689269	9781.568804	27.570765
265.459660	9789.847195	27.575783
265.880016	9811.681185	27.580800
265.751002	9826.783995	27.585818
266.108697	9840.446904	27.590836
266.175294	9859.867274	27.595853
266.372368	9888.440850	27.600871
266.977246	9887.562648	27.605888
267.168792	9910.311967	27.610906
267.419696	9915.984743	27.615924
267.466464	9945.691702	27.620941
267.540079	9969.915521	27.625959
268.080139	9980.193194	27.630976
268.327719	9996.461950	27.635994
268.841031	10010.223773	27.641012
268.908621	10033.081576	27.646029
269.268970	10064.965309	27.651047
269.448340	10070.356374	27.656064
269.503639	10098.869520	27.661082
269.779419	10116.256621	27.666100
270.288399	10135.355374	27.671117
270.408296	10157.996857	27.676135
270.884087	10167.491959	27.681152
270.954579	10203.243665	27.686170
271.167801	10214.772261	27.691188
271.623513	10241.109035	27.696205
271.595759	10259.617423	27.701223
272.092930	10265.746131	27.706240
272.001335	10290.831853	27.711258
272.327805	10310.461662	27.716276
272.758910	10336.421198	27.721293
273.234897	10359.833809	27.726311
273.698162	10367.945430	27.731328
273.905831	10388.511979	27.736346
274.306907	10402.552172	27.741364
275.004823	10425.632400	27.746381
274.651026	10434.890377	27.751399
275.418295	10438.724340	27.756416
275.290098	10453.810723	27.761434
275.921869	10466.587578	27.766452
276.351282	10480.310079	27.771469
276.953202	10486.452090	27.776487
277.397865	10494.981132	27.781504
277.522549	10512.850251	27.786522
277.819336	10516.341688	27.791540
278.115199	10519.999541	27.796557
277.982887	10522.174935	27.801575
278.707846	10527.775532	27.806592
278.519379	10544.019145	27.811610
278.789145	10553.257692	27.816628
278.883228	10547.715678	27.821645
279.123491	10569.545235	27.826663
279.514166	10572.816692	27.831680
279.481369	10588.466691	27.836698
279.799726	10603.126886	27.841716
280.209603	10611.888017	27.846733
280.185484	10630.444487	27.851751
280.861668	10639.567937	27.856768
280.622048	10654.270088	27.861786
281.011425	10671.863644	27.866804
281.210638	10691.058126	27.871821
281.335368	10711.333738	27.876839
281.865516	10716.336589	27.881856
281.905003	10756.467113	27.886874
282.001815	10763.468161	27.891892
282.477551	10791.634616	27.896909
282.534067	10823.872975	27.901927
283.143841	10830.509736	27.906944
282.905554	10861.092716	27.911962
283.122936	10891.049027	27.916980
283.356865	10913.226404	27.921997
283.776942	10941.130859	27.927015
284.385993	10959.368989	27.932032
284.722549	10993.407209	27.937050
284.905278	11003.619754	27.942068
285.465223	11027.722100	27.947085
285.770992	11054.067662	27.952103
286.142557	11065.943571	27.957120
286.391428	11087.104264	27.962138
286.872399	11106.129020	27.967156
286.816944	11127.082666	27.972173
286.974897	11148.903745	27.977191
287.505271	11163.479333	27.982208
287.387183	11187.935576	27.987226
287.699951	11209.858396	27.992244
288.392896	11230.698018	27.997261
288.861346	11253.267088	28.002279
289.771049	11258.799558	28.007296
290.013638	11261.697286	28.012314
290.485344	11271.313182	28.017332
291.010543	11286.958792	28.022349
290.761027	11296.865177	28.027367
291.159914	11288.364011	28.032384
291.239633	11304.597176	28.037402
291.683963	11305.676827	28.042420
291.884992	11311.645766	28.047437
291.959291	11326.212344	28.052455
292.213681	11324.205347	28.057472
292.409168	11341.660572	28.062490
292.730181	11364.695856	28.067508
292.788567	11374.965267	28.072525
292.982616	11407.570201	28.077543
293.429130	11425.727755	28.082560
293.485587	11451.271342	28.087578
293.649804	11466.703121	28.092596
294.145976	11484.968930	28.097613
293.934872	11510.776242	28.102631
294.455307	11530.573106	28.107648
294.418385	11557.411009	28.112666
294.983426	11579.413404	28.117684
295.582633	11597.206204	28.122701
295.641686	11622.524550	28.127719
295.995961	11632.848711	28.132736
296.095831	11661.787064	28.137754
296.377171	11683.806098	28.142772
296.934307	11707.299958	28.147789
296.777425	11737.408896	28.152807
297.045541	11756.615391	28.157824
297.734496	11776.784594	28.162842
298.118844	11804.546977	28.167860
298.487089	11826.446892	28.172877
298.709926	11846.945704	28.177895
299.362939	11856.118851	28.182912
299.163129	11882.094617	28.187930
299.726918	11903.555351	28.192948
300.088071	11922.621287	28.197965
300.330546	11939.307766	28.202983
300.718315	11961.899803	28.208000
300.921595	11979.919289	28.213018
301.233804	11994.093591	28.218036
301.636612	12009.343652	28.223053
301.843396	12033.792374	28.228071
302.768725	12044.810580	28.233088
302.783229	12080.195442	28.238106
302.679928	12097.667867	28.243124
303.210359	12112.255187	28.248141
303.156833	12138.924178	28.253159
303.413674	12156.089255	28.258176
303.532557	12178.465793	28.263194
304.162017	12209.154931	28.268212
304.866747	12235.742896	28.273229
304.805098	12254.338420	28.278247
305.617602	12262.780521	28.283264
305.749944	12279.591191	28.288282
305.592763	12297.787264	28.293300
306.201306	12320.655476	28.298317
306.501167	12349.852541	28.303335
306.721169	12367.256431	28.308352
307.120883	12386.601656	28.313370
307.469184	12398.613086	28.318388
307.816327	12416.086701	28.323405
307.477997	12442.543622	28.328423
308.195419	12463.516632	28.333440
308.610670	12479.709874	28.338458
308.668243	12506.664465	28.343476
309.325190	12517.363895	28.348493
309.041316	12550.864152	28.353511
309.360560	12577.262752	28.358528
310.175257	12599.102860	28.363546
310.522026	12617.770407	28.368564
311.154455	12619.925959	28.373581
311.342896	12649.336278	28.378599
311.829554	12645.680660	28.383616
312.200790	12663.109295	28.388634
312.026259	12677.934574	28.393652
312.381495	12685.634182	28.398669
312.481594	12705.601412	28.403687
312.774925	12720.008468	28.408704
313.162048	12749.812784	28.413722
313.634657	12764.981339	28.418740
314.256364	12784.639525	28.423757
314.299192	12802.437300	28.428775
314.578750	12814.865216	28.433792
314.678870	12829.861868	28.438810
314.795038	12850.191289	28.443828
315.224010	12872.189203	28.448845
315.865991	12896.347277	28.453863
315.837838	12911.746531	28.458880
316.152439	12932.851300	28.463898
316.069284	12964.876653	28.468916
316.832824	12976.579519	28.473933
317.394641	13002.380014	28.478951
317.814476	13011.672503	28.483968
318.173164	13028.374521	28.488986
318.072190	13060.217137	28.494004
318.574485	13068.114114	28.499021
318.759665	13095.688803	28.504039
319.316953	13122.805230	28.509056
319.506181	13134.983502	28.514074
319.814713	13166.533184	28.519092
320.132158	13187.050406	28.524109
320.288034	13212.700457	28.529127
320.570996	13235.432120	28.534144
321.035639	13250.358398	28.539162
321.685507	13272.493985	28.544180
322.257997	13282.772489	28.549197
322.597186	13306.181542	28.554215
322.979463	13315.576046	28.559232
322.982407	13332.655877	28.564250
323.455636	13345.704380	28.569268
324.029570	13361.219571	28.574285
324.191239	13385.512730	28.579303
324.282158	13396.549191	28.584320
324.621210	13420.790422	28.589338
324.853496	13428.277480	28.594356
325.057291	13457.313869	28.599373
324.986711	13477.692975	28.604391
325.439194	13497.475092	28.609408
325.605436	13527.197455	28.614426
325.733406	13554.372146	28.619444
326.494012	13582.959490	28.624461
326.771518	13615.213993	28.629479
326.753376	13632.120689	28.634496
327.293497	13656.265894	28.639514
327.105628	13683.241991	28.644532
327.613329	13709.563215	28.649549
328.410468	13734.086386	28.654567
328.720905	13754.134923	28.659584
329.349452	13767.863505	28.664602
329.201092	13799.217285	28.669620
330.089043	13810.328753	28.674637
330.842587	13818.150656	28.679655
331.128217	13825.137488	28.684672
331.469424	13830.081459	28.689690
331.812045	13850.179213	28.694708
332.290585	13858.934930	28.699725
332.235273	13872.856038	28.704743
332.431794	13891.928241	28.709760
332.766866	13895.668152	28.714778
332.827427	13929.853551	28.719796
333.396800	13934.426718	28.724813
333.601478	13960.910422	28.729831
333.472735	13984.776009	28.734848
333.753139	14004.632949	28.739866
334.092821	14036.606243	28.744884
334.797446	14047.538679	28.749901
334.888276	14076.635574	28.754919
335.349898	14093.127708	28.759936
335.895764	14119.742316	28.764954
335.947804	14146.454069	28.769972
336.084677	14165.714725	28.774989
336.864549	14189.915265	28.780007
336.979569	14226.843885	28.785024
337.559122	14232.699232	28.790042
337.901411	14265.682140	28.795060
338.526012	14281.131275	28.800077
338.555470	14298.196638	28.805095
338.897715	14326.924868	28.810112
339.376096	14335.343250	28.815130
339.440372	14366.995737	28.820148
340.040717	14372.255118	28.825165
340.529871	14400.189151	28.830183
340.613343	14425.615017	28.835200
341.138497	14442.253084	28.840218
341.205432	14470.495531	28.845236
342.047606	14478.805929	28.850253
342.336685	14510.258347	28.855271
342.375867	14524.949791	28.860288
342.709530	14546.927715	28.865306
342.638743	14570.696012	28.870324
343.188543	14588.308787	28.875341
343.701997	14612.188046	28.880359
343.566137	14648.676636	28.885376
343.981785	14672.473166	28.890394
344.650260	14689.449824	28.895412
345.102620	14712.612517	28.900429
345.445106	14743.474810	28.905447
345.841928	14763.677804	28.910464
345.961607	14786.148465	28.915482
345.790767	14818.793432	28.920500
346.295585	14832.295289	28.925517
346.706282	14864.225136	28.930535
346.876262	14888.947238	28.935552
347.318778	14917.770224	28.940570
347.861430	14941.917743	28.945588
348.265529	14963.462954	28.950605
348.503311	14988.018330	28.955623
348.785321	15017.231201	28.960640
349.038442	15035.848033	28.965658
349.375477	15074.985123	28.970676
350.402163	15081.222340	28.975693
351.131362	15096.448672	28.980711
351.337868	15117.119802	28.985728
351.608188	15123.276414	28.990746
352.072337	15129.232282	28.995764
351.962906	15154.086332	29.000781
352.374157	15174.083853	29.005799
352.623944	15194.053201	29.010816
353.185853	15208.829397	29.015834
353.825275	15222.323141	29.020852
354.019173	15247.891309	29.025869
354.527382	15258.775418	29.030887
354.482660	15281.351532	29.035904
355.264140	15294.014533	29.040922
355.486672	15316.980736	29.045940
355.682057	15330.415035	29.050957
355.715555	15355.578679	29.055975
355.919573	15385.591790	29.060992
356.673811	15391.966638	29.066010
356.585172	15432.889594	29.071028
356.628136	15456.069244	29.076045
357.286599	15490.785004	29.081063
357.222382	15523.744944	29.086080
357.837187	15549.852184	29.091098
358.391851	15591.704436	29.096116
358.648142	15613.577623	29.101133
359.020628	15649.089235	29.106151
359.193659	15671.686332	29.111168
360.225665	15696.547729	29.116186
360.390566	15722.197675	29.121204
360.950893	15735.712939	29.126221
361.267920	15769.995594	29.131239
361.571807	15789.584685	29.136256
362.259724	15816.169069	29.141274
362.243007	15846.360363	29.146292
362.386973	15857.390924	29.151309
362.973173	15892.273422	29.156327
362.960510	15931.153081	29.161344
363.478747	15947.904309	29.166362
363.923159	15968.999264	29.171380
365.193269	15979.802433	29.176397
365.597960	15997.444577	29.181415
365.857438	16021.926298	29.186432
366.581129	16024.618763	29.191450
366.618638	16033.207937	29.196468
366.735880	16040.245941	29.201485
366.836629	16056.826037	29.206503
367.276580	16089.023034	29.211520
367.409104	16094.535113	29.216538
367.555556	16119.727470	29.221556
367.743264	16141.114336	29.226573
368.474835	16166.487923	29.231591
368.449648	16202.099016	29.236608
368.597819	16214.182836	29.241626
368.735758	16251.658481	29.246644
369.223228	16281.074850	29.251661
369.854971	16311.882772	29.256679
369.981472	16340.738699	29.261696
370.590965	16368.188258	29.266714
370.608497	16405.810424	29.271732
371.113646	16429.461556	29.276749
371.608667	16463.516608	29.281767
371.641493	16507.627622	29.286784
371.733455	16542.472633	29.291802
372.461036	16578.869522	29.296820
372.813556	16613.179490	29.301837
373.477283	16648.080473	29.306855
373.551939	16687.518959	29.311872
374.165732	16707.862366	29.316890
374.460137	16745.572729	29.321908
375.182270	16782.833146	29.326925
375.449767	16811.880074	29.331943
375.838970	16849.948804	29.336960
376.425208	16878.068707	29.341978
376.407324	16910.648234	29.346996
376.934264	16943.339829	29.352013
377.324692	16970.905678	29.357031
377.657277	17011.341273	29.362048
378.380662	17041.170702	29.367066
378.766764	17069.736620	29.372084
378.745534	17101.823382	29.377101
379.619041	17133.474333	29.382119
379.787496	17159.340854	29.387136
380.343205	17190.487444	29.392154
380.449786	17218.642270	29.397172
381.006285	17245.505765	29.402189
381.419866	17273.854293	29.407207
381.459250	17313.597627	29.412224
382.365918	17339.528709	29.417242
383.058896	17349.960249	29.422260
383.848650	17364.559888	29.427277
384.995187	17362.653676	29.432295
385.280828	17370.422547	29.437312
385.749628	17367.039662	29.442330
385.686615	17375.294805	29.447348
386.438756	17390.667401	29.452365
386.739902	17395.342042	29.457383
386.742837	17400.085855	29.462400
386.904173	17399.054743	29.467418
387.140649	17417.049332	29.472436
387.582950	17432.812685	29.477453
387.642881	17439.575807	29.482471
387.700788	17466.708507	29.487488
387.957781	17484.519586	29.492506
388.208281	17502.280933	29.497524
388.370168	17535.644557	29.502541
388.901507	17554.946682	29.507559
388.978990	17589.501851	29.512576
389.578889	17622.971464	29.517594
390.011698	17647.568689	29.522612
389.961959	17688.241380	29.527629
390.565898	17708.799493	29.532647
390.457010	17750.712522	29.537664
391.047436	17785.567903	29.542682
391.301307	17828.513932	29.547700
391.730485	17865.420466	29.552717
392.173806	17906.239580	29.557735
392.442740	17949.233544	29.562752
393.171619	17985.078777	29.567770
393.280994	18028.177520	29.572788
394.038006	18065.903992	29.577805
394.435805	18102.160144	29.582823
394.569883	18139.352549	29.587840
395.226835	18176.654261	29.592858
395.671025	18212.467029	29.597876
396.250360	18241.913820	29.602893
396.763168	18270.801542	29.607911
397.108030	18317.437432	29.612928
397.940428	18340.484179	29.617946
398.651654	18361.095358	29.622964
399.035881	18380.852692	29.627981
399.594200	18405.079907	29.632999
399.628560	18421.545928	29.638016
400.353505	18443.016910	29.643034
400.691111	18463.577117	29.648052
401.087779	18486.126139	29.653069
401.692359	18506.410381	29.658087
401.466967	18528.284499	29.663104
401.836408	18545.116587	29.668122
402.706590	18559.171033	29.673140
402.717442	18587.151046	29.678157
403.581352	18603.919374	29.683175
403.442832	18635.089702	29.688192
404.128295	18657.694148	29.693210
404.612219	18675.381447	29.698228
404.942477	18713.892122	29.703245
405.360460	18729.508684	29.708263
405.398368	18763.470333	29.713280
405.737871	18791.066815	29.718298
406.936183	18796.915604	29.723316
407.354982	18812.542356	29.728333
407.715426	18839.322118	29.733351
407.970431	18866.387651	29.738368
408.139951	18886.373952	29.743386
408.410601	18900.861673	29.748404
408.519328	18927.659249	29.753421
409.009070	18950.773705	29.758439
409.361922	18974.228941	29.763456
409.525024	19013.214282	29.768474
410.137574	19030.753130	29.773492
410.207247	19061.094582	29.778509
410.829923	19094.201873	29.783527
411.028726	19129.165183	29.788544
411.442976	19153.559055	29.793562
412.252678	19181.462066	29.798580
412.465245	19218.444506	29.803597
412.911747	19240.955966	29.808615
413.136648	19277.179786	29.813632
413.614100	19313.379202	29.818650
414.144758	19339.433785	29.823668
414.252539	19376.326585	29.828685
414.873803	19410.366791	29.833703
415.031200	19446.880539	29.838720
415.544795	19480.870721	29.843738
416.331950	19496.613510	29.848756
416.853918	19537.706289	29.853773
417.390810	19559.280832	29.858791
417.815173	19593.108283	29.863808
418.476487	19611.618512	29.868826
419.101654	19628.031045	29.873844
419.352887	19657.138234	29.878861
420.006883	19676.239563	29.883879
420.319126	19703.162756	29.888896
420.579309	19724.893445	29.893914
421.133164	19739.334458	29.898932
421.073556	19772.080161	29.903949
421.934281	19793.238805	29.908967
421.690982	19831.068284	29.913984
421.823036	19857.777102	29.919002
422.641641	19888.979737	29.924020
422.797962	19930.232212	29.929037
423.498990	19964.026621	29.934055
423.630459	19998.424540	29.939072
423.961066	20022.881920	29.944090
424.329514	20064.190730	29.949108
424.434297	20110.586692	29.954125
425.151997	20148.807229	29.959143
425.446025	20188.512168	29.964160
426.666742	20194.687525	29.969178
428.818810	20187.505662	29.974196
429.650293	20201.117681	29.979213
430.306941	20193.403847	29.984231
430.737255	20197.260573	29.989248
431.185629	20188.593119	29.994266
431.598799	20175.773005	29.999284
431.408761	20166.263790	30.004301
431.681454	20170.312583	30.009319
431.600736	20192.998406	30.014336
431.715370	20204.697479	30.019354
432.081797	20207.060947	30.024372
432.025588	20225.996521	30.029389
432.270049	20246.856253	30.034407
432.617272	20280.791986	30.039424
432.723888	20295.986008	30.044442
433.531901	20326.028768	30.049460
433.273957	20364.382437	30.054477
433.884777	20392.746947	30.059495
434.140147	20418.103727	30.064512
434.245811	20465.035351	30.069530
434.614885	20501.730861	30.074548
434.961569	20551.331214	30.079565
435.085192	20585.889968	30.084583
435.765249	20634.867267	30.089600
435.979612	20679.703014	30.094618
436.523600	20727.122399	30.099636
436.657576	20776.910140	30.104653
437.495495	20824.742150	30.109671
438.351319	20862.145384	30.114688
439.304460	20879.467835	30.119706
440.208114	20913.664394	30.124724
440.597986	20948.550903	30.129741
441.220643	20969.545086	30.134759
441.288025	21004.626439	30.139776
441.439155	21033.378804	30.144794
442.364205	21058.674027	30.149812
442.752740	21095.597010	30.154829
442.771750	21123.594805	30.159847
443.665606	21154.743078	30.164864
443.530831	21187.605294	30.169882
444.230501	21223.627608	30.174900
444.436166	21263.117778	30.179917
444.763770	21294.062763	30.184935
445.291502	21328.453221	30.189952
445.601046	21366.981181	30.194970
446.138273	21406.158185	30.199988
446.287060	21457.637503	30.205005
446.701238	21496.533465	30.210023
447.261868	21533.028367	30.215040
447.837470	21576.520560	30.220058
448.458813	21616.253347	30.225076
448.830581	21655.113136	30.230093
449.236683	21690.182214	30.235111
449.666583	21735.567884	30.240128
450.088602	21778.058819	30.245146
450.795948	21810.543997	30.250164
451.144291	21856.465208	30.255181
451.689501	21886.056607	30.260199
452.196081	21917.297230	30.265216
452.373060	21968.737485	30.270234
452.796852	21998.043619	30.275252
453.151580	22042.337082	30.280269
453.549230	22076.630957	30.285287
454.162826	22128.143158	30.290304
454.390238	22170.572418	30.295322
455.251936	22199.865873	30.300340
455.616822	22242.382907	30.305357
455.798158	22267.443325	30.310375
456.738659	22298.546258	30.315392
456.798867	22341.422433	30.320410
457.311933	22367.812504	30.325428
457.667371	22417.852102	30.330445
458.209092	22443.497331	30.335463
458.861574	22483.740104	30.340480
458.918142	22523.474560	30.345498
459.591083	22554.366992	30.350516
459.979370	22596.074671	30.355533
460.468724	22638.006600	30.360551
461.101751	22665.695047	30.365568
461.417438	22711.052868	30.370586
462.276155	22743.697013	30.375604
462.262082	22791.528138	30.380621
462.670995	22837.244828	30.385639
463.028867	22870.017071	30.390656
463.330921	22915.632070	30.395674
464.159496	22948.205820	30.400692
464.663850	22997.735151	30.405709
464.945171	23045.089109	30.410727
465.696063	23085.926619	30.415744
465.788268	23125.471003	30.420762
466.435698	23167.862793	30.425780
466.939732	23217.272340	30.430797
467.362727	23255.281891	30.435815
468.245498	23292.972524	30.440832
469.680961	23309.548121	30.445850
471.202531	23304.520524	30.450868
471.613683	23331.429417	30.455885
471.606565	23351.410125	30.460903
471.909477	23360.508089	30.465920
472.322532	23382.681841	30.470938
472.924110	23398.121373	30.475956
473.237735	23423.150723	30.480973
473.078458	23447.952965	30.485991
473.548588	23473.326111	30.491008
473.683963	23506.840117	30.496026
474.167004	23538.628056	30.501044
474.492603	23577.677141	30.506061
474.936676	23617.183233	30.511079
475.332712	23655.263416	30.516096
475.282645	23700.739037	30.521114
475.995722	23732.790842	30.526132
475.932442	23785.298498	30.531149
476.271702	23830.867651	30.536167
476.864334	23872.259385	30.541184
477.230805	23946.486303	30.546202
477.616807	23996.688265	30.551220
478.001407	24053.965336	30.556237
478.284452	24111.121722	30.561255
478.862120	24170.871914	30.566272
479.241913	24224.306141	30.571290
479.734753	24277.769016	30.576308
480.366537	24331.603813	30.581325
481.166810	24380.014218	30.586343
481.820736	24421.958496	30.591360
482.338184	24469.075029	30.596378
483.203347	24502.678895	30.601396
484.031654	24537.706685	30.606413
484.489914	24573.086550	30.611431
484.636425	24612.013862	30.616448
485.301512	24654.392610	30.621466
485.682555	24689.882718	30.626484
486.016749	24737.601947	30.631501
486.368067	24768.037068	30.636519
487.257925	24814.361871	30.641536
487.313352	24864.510499	30.646554
487.729603	24899.855238	30.651572
488.333851	24943.519868	30.656589
488.704262	24985.237424	30.661607
489.244324	25033.387958	30.666624
489.662740	25072.883611	30.671642
490.377297	25120.132945	30.676660
491.016851	25163.514457	30.681677
491.331467	25209.995063	30.686695
492.012140	25263.448635	30.691712
492.285137	25306.192506	30.696730
492.764711	25341.487165	30.701748
494.119807	25376.947316	30.706765
494.505041	25420.971923	30.711783
495.224681	25444.480731	30.716800
495.479443	25482.701996	30.721818
496.110325	25513.283861	30.726836
496.990401	25536.801913	30.731853
497.535351	25565.229494	30.736871
498.297708	25593.316820	30.741888
498.577079	25618.383420	30.746906
499.272901	25644.612724	30.751924
499.594841	25658.379180	30.756941
499.876774	25688.848372	30.761959
500.538438	25710.554812	30.766976
500.934038	25738.904075	30.771994
501.458320	25773.928642	30.777012
501.415190	25798.372514	30.782029
501.895650	25842.890471	30.787047
502.685455	25882.005155	30.792064
502.789748	25925.553562	30.797082
503.036678	25956.491296	30.802100
503.953180	25998.497929	30.807117
503.850144	26042.572865	30.812135
504.429167	26095.501787	30.817152
504.955501	26138.573862	30.822170
505.529228	26180.359825	30.827188
505.532600	26222.799274	30.832205
506.137940	26283.496765	30.837223
506.792168	26324.559635	30.842240
506.970437	26389.022169	30.847258
507.183010	26425.636493	30.852276
507.497651	26477.090572	30.857293
507.814577	26529.415831	30.862311
508.707750	26582.697332	30.867328
508.871313	26644.085813	30.872346
509.568275	26690.323846	30.877364
510.238043	26747.457934	30.882381
510.639249	26804.475853	30.887399
511.199095	26850.632185	30.892416
512.607544	26884.726507	30.897434
514.112565	26908.616604	30.902452
514.719240	26938.278484	30.907469
515.162802	26962.074586	30.912487
516.162327	26984.203238	30.917504
516.707892	27009.967064	30.922522
517.413886	27025.261111	30.927540
517.817214	27042.599897	30.932557
517.770121	27065.620234	30.937575
518.399756	27084.027641	30.942592
518.875698	27121.881128	30.947610
519.083443	27145.426693	30.952628
519.796356	27180.570031	30.957645
519.899147	27210.336310	30.962663
520.392867	27239.202049	30.967680
520.394219	27285.325672	30.972698
520.950688	27324.908070	30.977716
521.155736	27371.105070	30.982733
521.657539	27416.807401	30.987751
522.521000	27442.872689	30.992768
522.807985	27487.418117	30.997786
523.718835	27536.345951	31.002804
524.091478	27577.316610	31.007821
524.608062	27622.295436	31.012839
525.744888	27659.840053	31.017856
525.700656	27710.072480	31.022874
526.696648	27742.626960	31.027892
527.195039	27781.159178	31.032909
527.482346	27826.471349	31.037927
528.001055	27857.734241	31.042944
528.370118	27899.199527	31.047962
528.744089	27948.078596	31.052980
529.345226	27986.235637	31.057997
530.010126	28029.252068	31.063015
530.533968	28061.414360	31.068032
531.129376	28110.740866	31.073050
531.649027	28157.302873	31.078068
532.181090	28189.393194	31.083085
532.321528	28250.608632	31.088103
533.043715	28289.136351	31.093120
533.643923	28339.868491	31.098138
534.216489	28396.603112	31.103156
534.824100	28434.890977	31.108173
535.178247	28473.001827	31.113191
535.682285	28519.116644	31.118208
536.263369	28566.052985	31.123226
536.664932	28602.241833	31.128244
537.253145	28642.714366	31.133261
537.336522	28680.883013	31.138279
538.053400	28725.642301	31.143296
538.644590	28773.988101	31.148314
538.979594	28820.702764	31.153332
539.559193	28867.436912	31.158349
539.846689	28921.170864	31.163367
540.375445	28960.180131	31.168384
540.838293	29016.143249	31.173402
541.266420	29073.979621	31.178420
542.248841	29129.753205	31.183437
542.488059	29183.632820	31.188455
543.222452	29234.073726	31.193472
543.953608	29278.906331	31.198490
545.089907	29310.700895	31.203508
545.803504	29352.452268	31.208525
546.257509	29403.901297	31.213543
546.817255	29434.360070	31.218560
547.587203	29481.705521	31.223578
547.896839	29518.010330	31.228596
548.609195	29551.147889	31.233613
549.167445	29589.457361	31.238631
549.834933	29626.234960	31.243648
550.326367	29666.165958	31.248666
550.613992	29703.035752	31.253684
551.053006	29750.617512	31.258701
551.329327	29797.810822	31.263719
551.704222	29831.165030	31.268736
552.195109	29887.405625	31.273754
552.789708	29943.064088	31.278772
553.522366	29994.366572	31.283789
553.595435	30045.079223	31.288807
554.596196	30105.385998	31.293824
554.799041	30156.867939	31.298842
555.132133	30219.541575	31.303860
555.913198	30271.158737	31.308877
556.112502	30334.815537	31.313895
557.222265	30390.888365	31.318912
557.884001	30439.539923	31.323930
558.199164	30490.406098	31.328948
559.202904	30538.210693	31.333965
559.387965	30599.322204	31.338983
559.882969	30659.273407	31.344000
560.645729	30717.011845	31.349018
560.884220	30769.575983	31.354036
561.734504	30828.378952	31.359053
562.411881	30884.927404	31.364071
563.018794	30936.237098	31.369088
563.448693	30992.744952	31.374106
563.760133	31049.275018	31.379124
564.612580	31084.409286	31.384141
564.869562	31147.956016	31.389159
566.522523	31178.820802	31.394176
569.393319	31145.602862	31.399194
570.459421	31154.128955	31.404212
570.986000	31147.121070	31.409229
571.386451	31158.552468	31.414247
571.837228	31161.809683	31.419264
572.134520	31153.783849	31.424282
572.307749	31166.017463	31.429300
573.005536	31158.925564	31.434317
572.980087	31167.696437	31.439335
573.279770	31182.044068	31.444352
573.417959	31199.716378	31.449370
573.940780	31225.031831	31.454388
574.540485	31233.499848	31.459405
574.596648	31282.002890	31.464423
575.342586	31304.089573	31.469440
575.573128	31332.846857	31.474458
575.593366	31384.415313	31.479476
576.285411	31422.562751	31.484493
576.122532	31480.504885	31.489511
576.664276	31529.151987	31.494528
577.188147	31590.030374	31.499546
577.528590	31649.087712	31.504564
578.183915	31710.087466	31.509581
578.401521	31775.781832	31.514599
578.854540	31845.616008	31.519616
579.645968	31918.886399	31.524634
579.765581	31993.186219	31.529652
580.809194	32055.719005	31.534669
581.008357	32132.035428	31.539687
581.606218	32210.810749	31.544704
582.413220	32276.603964	31.549722
582.754784	32351.935611	31.554740
583.865705	32419.600915	31.559757
584.430184	32500.080599	31.564775
585.032987	32557.776875	31.569792
585.889421	32621.742951	31.574810
586.558479	32686.760572	31.579828
587.306182	32738.464869	31.584845
587.862243	32802.632384	31.589863
588.423135	32860.722591	31.594880
590.110132	32902.362643	31.599898
591.117643	32935.545148	31.604916
592.180397	32965.503171	31.609933
592.805514	33004.921273	31.614951
593.332473	33040.180911	31.619968
594.234281	33068.906822	31.624986
594.008486	33101.447448	31.630004
594.664040	33134.377437	31.635021
595.197055	33177.184038	31.640039
595.532087	33217.282543	31.645056
595.945027	33266.853797	31.650074
596.472830	33306.423682	31.655092
597.274568	33356.814485	31.660109
597.536446	33406.864212	31.665127
598.007685	33457.249626	31.670144
598.714726	33497.622183	31.675162
599.015746	33542.224355	31.680180
599.464354	33582.338757	31.685197
600.224027	33637.687029	31.690215
600.523090	33683.404415	31.695232
601.153345	33733.051223	31.700250
601.552642	33781.035572	31.705268
602.256244	33829.126088	31.710285
602.584786	33892.705049	31.715303
603.020347	33946.417599	31.720320
604.082185	34008.863420	31.725338
604.473641	34071.220754	31.730356
604.991879	34121.622762	31.735373
605.754626	34194.650806	31.740391
606.457820	34248.346931	31.745408
607.108001	34296.322763	31.750426
607.524567	34349.125279	31.755444
608.382915	34415.374392	31.760461
608.437939	34479.256109	31.765479
609.379009	34542.133048	31.770496
609.967259	34597.918544	31.775514
610.748521	34668.940402	31.780532
611.789184	34706.614226	31.785549
612.842048	34761.099752	31.790567
613.671399	34788.381901	31.795584
614.498099	34828.357112	31.800602
615.032160	34877.135061	31.805620
615.754762	34913.266133	31.810637
616.297886	34952.654610	31.815655
616.413767	34993.675145	31.820672
617.337724	35038.614086	31.825690
617.685467	35092.356917	31.830708
618.411824	35139.536342	31.835725
618.852488	35187.458235	31.840743
619.390729	35236.742641	31.845760
619.773518	35286.922213	31.850778
620.321221	35353.451538	31.855796
620.965224	35397.275666	31.860813
621.203113	35457.132210	31.865831
621.732563	35524.704089	31.870848
622.905238	35584.755928	31.875866
622.848302	35646.794806	31.880884
623.430648	35726.481566	31.885901
624.124788	35786.615059	31.890919
624.660429	35849.780623	31.895936
625.492795	35910.376570	31.900954
625.912834	35984.633697	31.905972
626.726486	36035.211999	31.910989
627.415487	36114.304986	31.916007
628.175235	36171.033314	31.921024
629.027792	36231.411203	31.926042
629.434978	36296.062033	31.931060
629.971291	36354.527778	31.936077
630.790042	36419.089893	31.941095
631.122618	36487.824311	31.946112
632.368289	36529.663569	31.951130
633.211108	36577.594759	31.956148
634.137228	36620.677105	31.961165
634.845122	36656.967218	31.966183
635.140107	36713.944820	31.971200
635.906597	36745.049483	31.976218
636.383079	36797.619960	31.981236
636.850843	36840.492049	31.986253
637.431017	36885.799719	31.991271
637.723917	36946.567290	31.996288
638.427274	37005.860124	32.001306
638.748432	37057.251522	32.006324
639.543818	37114.576512	32.011341
639.968054	37180.073145	32.016359
640.189012	37255.736180	32.021376
641.190991	37310.894017	32.026394
641.624468	37382.214501	32.031412
641.959512	37450.971363	32.036429
642.588759	37514.845686	32.041447
643.003875	37597.273656	32.046464
643.635995	37677.855739	32.051482
643.813674	37763.993095	32.056500
644.660066	37841.303091	32.061517
645.756622	37923.505878	32.066535
646.167136	38004.875364	32.071552
647.306850	38067.528867	32.076570
647.924567	38151.392139	32.081588
648.502023	38218.856774	32.086605
649.343545	38294.923908	32.091623
650.100235	38371.350222	32.096640
650.720931	38438.335787	32.101658
651.380379	38522.779261	32.106676
652.485139	38575.920653	32.111693
653.349035	38641.661986	32.116711
653.636661	38717.292529	32.121728
654.517903	38774.103279	32.126746
654.988465	38848.757564	32.131764
655.490325	38907.576640	32.136781
656.237568	38981.652881	32.141799
656.891818	39054.200448	32.146816
657.825207	39120.593294	32.151834
657.812605	39192.243128	32.156852
658.805705	39269.738106	32.161869
659.549293	39330.805135	32.166887
660.287507	39408.071669	32.171904
661.510507	39457.440693	32.176922
662.561623	39521.392576	32.181940
663.080987	39575.412474	32.186957
663.982819	39636.427016	32.191975
665.157095	39671.110201	32.196992
666.841070	39681.060995	32.202010
667.443151	39726.211907	32.207028
667.907775	39748.625801	32.212045
669.277441	39780.881090	32.217063
669.852394	39807.696209	32.222080
670.434637	39833.377930	32.227098
671.005562	39840.292139	32.232116
671.528426	39862.428823	32.237133
671.756367	39892.305076	32.242151
671.959741	39919.766177	32.247168
672.660483	39941.196532	32.252186
672.650814	39986.111211	32.257204
672.983561	40028.136028	32.262221
673.566760	40074.688097	32.267239
673.734514	40138.161602	32.272256
674.206768	40193.023620	32.277274
674.548521	40260.428201	32.282292
675.053837	40327.756538	32.287309
675.620059	40392.615258	32.292327
676.492017	40468.676203	32.297344
677.284414	40538.943436	32.302362
677.830124	40613.836330	32.307380
678.419865	40686.435790	32.312397
679.008739	40759.732762	32.317415
679.317494	40846.186509	32.322432
680.216277	40925.001946	32.327450
680.913396	41007.114445	32.332468
681.658774	41086.106447	32.337485
682.084598	41163.670359	32.342503
683.150326	41243.523649	32.347520
683.932464	41318.867721	32.352538
684.547770	41406.666499	32.357556
685.307284	41478.519942	32.362573
685.800649	41541.725981	32.367591
686.493560	41633.980039	32.372608
687.333994	41716.420075	32.377626
688.192593	41798.602112	32.382644
688.813089	41887.241563	32.387661
689.599998	41951.077397	32.392679
690.236199	42032.037361	32.397696
691.162175	42114.371047	32.402714
691.655847	42188.916313	32.407732
692.246944	42275.669790	32.412749
693.136009	42344.572596	32.417767
693.588932	42436.272957	32.422784
694.338595	42510.747308	32.427802
694.975937	42591.255463	32.432820
695.900606	42671.907516	32.437837
697.045855	42733.045716	32.442855
697.896262	42806.678819	32.447872
699.427505	42841.153871	32.452890
700.730685	42897.213953	32.457908
701.680976	42944.062334	32.462925
702.324969	42992.249822	32.467943
703.172376	43035.171634	32.472960
703.654571	43084.435608	32.477978
704.041873	43136.853640	32.482996
704.649396	43182.082154	32.488013
705.219508	43234.439830	32.493031
705.552662	43295.185645	32.498048
706.203818	43342.461283	32.503066
706.659559	43402.090148	32.508084
707.311881	43454.422780	32.513101
708.280318	43499.250804	32.518119
708.421785	43569.182889	32.523136
709.033525	43619.206957	32.528154
709.596482	43689.249081	32.533172
709.936197	43749.985975	32.538189
710.657533	43823.542993	32.543207
711.197951	43904.205164	32.548224
711.949376	43976.171210	32.553242
712.569435	44043.353787	32.558260
712.841552	44132.180049	32.563277
713.891595	44198.401969	32.568295
714.427861	44286.615950	32.573312
715.125692	44362.989904	32.578330
715.830451	44456.134115	32.583348
716.581574	44534.175544	32.588365
717.271590	44614.974925	32.593383
718.298343	44698.573069	32.598400
718.978518	44765.796177	32.603418
720.055618	44850.579576	32.608436
720.625807	44935.144372	32.613453
721.824289	44998.367464	32.618471
722.398778	45076.429969	32.623488
723.171274	45153.748281	32.628506
723.812933	45232.901867	32.633524
724.794249	45307.354457	32.638541
725.530801	45370.381106	32.643559
725.856935	45448.667796	32.648576
726.430992	45524.315633	32.653594
727.942371	45592.494914	32.658612
729.324262	45646.222919	32.663629
730.367093	45708.088297	32.668647
731.102951	45775.312726	32.673664
731.780604	45833.450611	32.678682
732.611429	45875.148430	32.683700
733.393315	45935.857224	32.688717
734.006215	45992.362143	32.693735
734.193493	46046.849474	32.698752
735.242392	46095.861349	32.703770
736.025020	46162.906285	32.708788
736.239809	46240.157257	32.713805
737.089739	46298.805630	32.718823
737.597934	46372.082306	32.723840
738.264938	46439.591581	32.728858
738.808080	46510.118263	32.733876
739.283105	46580.372102	32.738893
740.027537	46652.656311	32.743911
740.620113	46740.624398	32.748928
741.049315	46815.871736	32.753946
741.832036	46906.378749	32.758964
742.241548	46997.213835	32.763981
743.048191	47086.809244	32.768999
743.321107	47178.878641	32.774016
744.529945	47266.394690	32.779034
745.394414	47344.619876	32.784052
745.703256	47433.699928	32.789069
746.695219	47509.633692	32.794087
747.216023	47605.386023	32.799104
747.844641	47679.702848	32.804122
748.970838	47761.119339	32.809140
749.978185	47837.951355	32.814157
752.227179	47877.187806	32.819175
753.677245	47930.271390	32.824192
754.569663	47974.921027	32.829210
755.549504	48024.703416	32.834228
755.982072	48063.945446	32.839245
756.897161	48104.016374	32.844263
757.314480	48167.608718	32.849280
757.622276	48222.377024	32.854298
758.164067	48277.108250	32.859316
758.605530	48340.691059	32.864333
759.212990	48399.429181	32.869351
759.909758	48474.079283	32.874368
760.367277	48544.952720	32.879386
761.044050	48620.158840	32.884404
761.256018	48703.000036	32.889421
762.241561	48784.506728	32.894439
762.951484	48862.182579	32.899456
763.761948	48944.333216	32.904474
765.425345	49013.407195	32.909492
765.862624	49095.766249	32.914509
767.000097	49154.760150	32.919527
767.573891	49228.621985	32.924544
768.465537	49303.099381	32.929562
769.503919	49359.793461	32.934580
769.861946	49433.333895	32.939597
770.756271	49509.354867	32.944615
771.508726	49584.022844	32.949632
772.130442	49658.446862	32.954650
772.872589	49734.489859	32.959668
773.412723	49812.906922	32.964685
774.439153	49892.111607	32.969703
775.131395	49969.410083	32.974720
775.465411	50052.083468	32.979738
776.421886	50134.411998	32.984756
777.048166	50226.131620	32.989773
778.124514	50304.130959	32.994791
778.673871	50385.963704	32.999808
779.247578	50481.735680	33.004826
780.162528	50561.320840	33.009844
780.612432	50652.527899	33.014861
781.544380	50726.209508	33.019879
782.724587	50809.928853	33.024896
784.062865	50886.617185	33.029914
785.878652	50935.334168	33.034932
786.521737	51002.287018	33.039949
787.620775	51054.085039	33.044967
788.477484	51115.383483	33.049984
789.225096	51164.697177	33.055002
790.446634	51202.018436	33.060020
791.282803	51246.113983	33.065037
791.839744	51272.532952	33.070055
792.435989	51308.833571	33.075072
792.941724	51362.011427	33.080090
793.473352	51403.236489	33.085108
793.835304	51464.741118	33.090125
794.618988	51518.960882	33.095143
795.102534	51596.473164	33.100160
795.408090	51663.463261	33.105178
796.238642	51727.895651	33.110196
796.517551	51803.648722	33.115213
797.568168	51876.246229	33.120231
798.049634	51967.467544	33.125248
798.761553	52045.529290	33.130266
799.597755	52129.953390	33.135284
800.409922	52211.746286	33.140301
801.160109	52304.381534	33.145319
801.523366	52386.262451	33.150336
802.279348	52486.867184	33.155354
803.245819	52584.118585	33.160372
803.659587	52679.993967	33.165389
804.654994	52776.197064	33.170407
805.333406	52878.426025	33.175424
806.413183	52966.473419	33.180442
807.915112	53051.635436	33.185460
808.973738	53132.702021	33.190477
810.422620	53202.182950	33.195495
811.582738	53284.506077	33.200512
812.199571	53352.374533	33.205530
813.342530	53408.019970	33.210548
814.279382	53485.796447	33.215565
815.057633	53559.599303	33.220583
815.784916	53626.311731	33.225600
816.684153	53692.283677	33.230618
817.419251	53755.229686	33.235636
818.143103	53828.401528	33.240653
818.975607	53891.963802	33.245671
820.063050	53966.710234	33.250688
820.189500	54042.894626	33.255706
821.398223	54114.333274	33.260724
821.705803	54188.901712	33.265741
822.057320	54275.647756	33.270759
822.856828	54358.241466	33.275776
823.208123	54445.329258	33.280794
824.727229	54530.804816	33.285812
825.327935	54633.128590	33.290829
825.945835	54714.367058	33.295847
826.697365	54804.584211	33.300864
826.940297	54894.036770	33.305882
828.052622	54977.694633	33.310900
829.229399	55074.708047	33.315917
830.150625	55158.977985	33.320935
831.194084	55253.387185	33.325952
832.093315	55335.038196	33.330970
833.733250	55402.549407	33.335988
834.485054	55462.657563	33.341005
835.357348	55520.666431	33.346023
836.325568	55587.751737	33.351040
836.464956	55672.890310	33.356058
837.166087	55736.006381	33.361076
838.099392	55814.465729	33.366093
838.431753	55892.484392	33.371111
839.233394	55975.107144	33.376128
839.898600	56070.354169	33.381146
840.543645	56148.403072	33.386164
840.804885	56252.333600	33.391181
841.262235	56351.835924	33.396199
842.639742	56450.633565	33.401216
842.987936	56562.977840	33.406234
843.636238	56666.504987	33.411252
844.362695	56779.374414	33.416269
845.168977	56895.335159	33.421287
846.248712	57008.771691	33.426304
847.017125	57128.174761	33.431322
848.409025	57235.031079	33.436340
849.560019	57350.314715	33.441357
850.187043	57442.102093	33.446375
851.359063	57536.717204	33.451392
852.224141	57648.010248	33.456410
853.119185	57752.362933	33.461428
854.263829	57847.564902	33.466445
855.138121	57948.029205	33.471463
856.111046	58039.227765	33.476480
857.771388	58137.067496	33.481498
858.650212	58223.261966	33.486516
859.171348	58306.855360	33.491533
860.499593	58394.377759	33.496551
861.795313	58467.937980	33.501568
862.404161	58559.449612	33.506586
863.259137	58641.510614	33.511604
864.037828	58721.314008	33.516621
864.779568	58805.632287	33.521639
865.521246	58893.771339	33.526656
866.186060	58979.908646	33.531674
866.970138	59059.643168	33.536692
867.747746	59157.249856	33.541709
868.637737	59250.200945	33.546727
869.842478	59337.677966	33.551744
870.352323	59439.073432	33.556762
870.950362	59529.041231	33.561780
872.301803	59632.469823	33.566797
872.695168	59726.758982	33.571815
874.459771	59797.218647	33.576832
875.281058	59890.749041	33.581850
876.479579	59973.477973	33.586868
877.295984	60056.435427	33.591885
878.062105	60143.013490	33.596903
879.139924	60212.643062	33.601920
879.810934	60292.606067	33.606938
880.475464	60374.948109	33.611956
881.540522	60439.130551	33.616973
882.078630	60510.807986	33.621991
883.248643	60592.783200	33.627008
883.419718	60672.821062	33.632026
884.678180	60750.453764	33.637044
885.613075	60825.179543	33.642061
886.301549	60901.068966	33.647079
887.427761	60983.090744	33.652096
887.877495	61065.874172	33.657114
888.984728	61149.377500	33.662132
889.999451	61235.958922	33.667149
890.506255	61315.418742	33.672167
891.444176	61397.412287	33.677184
892.347474	61503.338177	33.682202
893.255202	61581.469047	33.687220
894.023948	61672.904089	33.692237
894.604456	61772.238823	33.697255
895.900076	61853.918488	33.702272
896.430346	61949.974839	33.707290
897.470141	62044.570609	33.712308
898.386273	62147.248611	33.717325
899.240953	62243.160088	33.722343
900.608817	62335.191414	33.727360
901.213525	62436.995270	33.732378
902.155306	62534.356482	33.737396
903.251938	62624.806029	33.742413
904.293242	62707.894084	33.747431
905.550719	62799.120994	33.752448
906.530442	62889.299867	33.757466
907.392986	62973.380722	33.762484
908.222489	63065.340194	33.767501
908.886474	63161.772988	33.772519
910.121182	63232.345617	33.777536
910.785724	63340.356700	33.782554
911.523194	63433.431605	33.787572
912.395950	63533.736470	33.792589
912.969640	63628.025836	33.797607
914.112238	63711.020039	33.802624
914.864567	63813.875212	33.807642
915.711495	63916.741150	33.812660
916.370977	64018.816337	33.817677
917.586736	64119.451838	33.822695
919.162834	64209.633645	33.827712
919.954661	64302.331459	33.832730
920.953354	64393.724028	33.837748
921.915862	64492.175214	33.842765
922.396254	64588.897076	33.847783
923.040664	64684.699527	33.852800
923.725122	64797.396266	33.857818
924.619341	64908.749578	33.862836
925.538098	65015.823210	33.867853
926.180195	65139.358711	33.872871
927.496178	65244.039524	33.877888
927.779309	65363.533979	33.882906
929.220417	65452.413415	33.887924
930.600438	65527.137358	33.892941
931.825338	65631.506293	33.897959
932.853923	65707.540764	33.902976
933.655266	65800.228491	33.907994
934.480860	65889.691130	33.913012
935.470582	65983.682652	33.918029
936.189370	66080.465663	33.923047
936.997841	66174.177414	33.928064
937.625871	66269.472342	33.933082
938.298553	66374.072131	33.938100
939.311171	66484.929278	33.943117
940.186353	66591.165759	33.948135
941.005178	66700.260877	33.953152
941.696007	66809.667570	33.958170
942.301815	66926.877688	33.963188
943.621771	67037.588016	33.968205
944.779227	67140.074289	33.973223
945.968803	67254.110602	33.978240
946.851209	67366.231720	33.983258
947.717929	67478.545504	33.988276
949.146017	67588.736366	33.993293
949.555170	67702.330895	33.998311
950.466673	67818.196317	34.003328
951.391259	67939.076576	34.008346
952.886865	68052.544507	34.013364
953.827456	68161.615806	34.018381
954.414128	68288.673885	34.023399
955.784340	68396.673614	34.028416
956.216266	68513.661902	34.033434
956.891270	68634.143917	34.038452
958.628680	68737.620356	34.043469
959.865010	68861.710451	34.048487
960.956528	68968.121322	34.053504
961.811779	69068.170190	34.058522
962.888993	69181.382699	34.063540
963.915309	69286.068198	34.068557
964.712719	69402.403415	34.073575
966.046047	69508.109019	34.078592
966.750642	69621.705574	34.083610
967.442235	69730.799943	34.088628
968.290994	69840.754471	34.093645
969.153615	69963.855829	34.098663
969.947262	70078.496008	34.103680
970.713071	70194.354414	34.108698
971.655194	70327.384229	34.113716
972.594898	70452.915289	34.118733
973.200732	70580.263129	34.123751
974.561107	70703.479461	34.128768
975.437330	70832.112801	34.133786
976.130601	70967.296919	34.138804
977.682685	71084.412909	34.143821
978.589043	71215.223885	34.148839
980.404408	71312.780822	34.153856
981.714990	71417.817844	34.158874
982.696321	71512.058394	34.163892
983.897395	71600.533242	34.168909
984.813894	71706.114717	34.173927
985.654994	71796.195829	34.178944
987.049277	71879.415449	34.183962
987.663238	71977.798682	34.188980
988.829864	72061.421782	34.193997
989.218685	72167.550937	34.199015
990.162545	72265.883110	34.204032
990.826105	72375.438824	34.209050
991.563946	72491.656316	34.214068
992.655061	72592.892428	34.219085
993.396853	72719.903742	34.224103
994.469986	72836.613350	34.229120
995.485192	72952.941059	34.234138
996.041547	73075.965076	34.239156
997.726074	73185.874672	34.244173
998.416924	73301.952680	34.249191
999.638493	73415.482358	34.254208
1000.862383	73529.859117	34.259226
1001.564690	73644.129918	34.264244
1002.662915	73763.286573	34.269261
1003.475917	73889.295478	34.274279
1004.391600	74004.406481	34.279296
1005.214998	74123.994488	34.284314
1006.324824	74256.669930	34.289332
1007.400550	74378.936772	34.294349
1008.757981	74504.072949	34.299367
1010.717593	74606.640927	34.304384
1011.811538	74721.228404	34.309402
1012.939616	74823.234583	34.314420
1014.292983	74913.014377	34.319437
1015.489670	75019.769510	34.324455
1017.005842	75103.229615	34.329472
1017.778202	75200.920887	34.334490
1018.429621	75301.159871	34.339508
1019.372809	75398.982925	34.344525
1020.109000	75503.684012	34.349543
1021.628745	75595.475434	34.354560
1022.717838	75695.823710	34.359578
1023.313789	75795.069059	34.364596
1024.272711	75893.328085	34.369613
1024.928253	76017.182193	34.374631
1026.228472	76121.853628	34.379648
1027.208536	76216.059564	34.384666
1028.153050	76337.436343	34.389684
1028.929924	76435.847035	34.394701
1029.637296	76548.900963	34.399719
1030.275753	76672.603763	34.404736
1031.541466	76798.590352	34.409754
1032.048416	76931.524566	34.414772
1032.888875	77050.387612	34.419789
1033.715613	77191.293422	34.424807
1034.537070	77318.472627	34.429824
1035.341918	77454.055435	34.434842
1036.222726	77590.695257	34.439860
1037.492691	77702.882302	34.444877
1038.594453	77840.765435	34.449895
1040.275117	77950.549814	34.454912
1041.141591	78076.045216	34.459930
1042.156041	78189.754649	34.464948
1043.661429	78306.806246	34.469965
1044.781012	78424.602542	34.474983
1046.055366	78535.238479	34.480000
1048.218434	78634.747687	34.485018
1049.594226	78722.796095	34.490036
1050.862650	78811.430856	34.495053
1051.808345	78899.617965	34.500071
1052.406309	79005.970845	34.505088
1053.478249	79095.447188	34.510106
1054.336776	79198.339856	34.515124
1055.449616	79297.924506	34.520141
1056.402646	79401.138178	34.525159
1057.261794	79508.090544	34.530176
1058.234656	79619.165849	34.535194
1058.758466	79736.052981	34.540212
1059.726556	79846.302163	34.545229
1060.785473	79966.165037	34.550247
1061.880160	80086.509668	34.555264
1063.062836	80205.241658	34.560282
1063.426608	80333.561620	34.565300
1064.615634	80457.604146	34.570317
1065.187744	80598.257634	34.575335
1065.835052	80738.659887	34.580352
1067.452051	80870.286028	34.585370
1068.053262	81017.809422	34.590388
1069.312459	81153.009156	34.595405
1070.647633	81288.659176	34.600423
1072.037585	81441.351488	34.605440
1072.937239	81575.934703	34.610458
1073.704116	81727.198296	34.615476
1075.283677	81854.822143	34.620493
1075.978832	82001.711646	34.625511
1076.863059	82154.122910	34.630528
1078.047970	82297.023200	34.635546
1079.377045	82439.572780	34.640564
1080.621036	82576.244540	34.645581
1081.790651	82717.525308	34.650599
1082.923843	82855.607404	34.655616
1084.094174	82999.564288	34.660634
1085.120612	83147.212032	34.665652
1086.501319	83273.156424	34.670669
1087.474622	83409.389810	34.675687
1088.783125	83542.257761	34.680704
1090.370338	83661.058791	34.685722
1091.543132	83792.691712	34.690740
1092.783918	83916.386058	34.695757
1094.031568	84031.563405	34.700775
1094.779240	84154.351231	34.705792
1096.083128	84273.200759	34.710810
1096.678416	84400.724683	34.715828
1098.060177	84499.165832	34.720845
1099.185010	84617.830790	34.725863
1100.245661	84722.533072	34.730880
1101.101752	84836.449257	34.735898
1102.094891	84959.582066	34.740916
1102.901431	85072.166927	34.745933
1103.753233	85206.901007	34.750951
1104.679404	85334.599200	34.755968
1105.681485	85462.248145	34.760986
1106.550608	85596.868113	34.766004
1107.463772	85716.963937	34.771021
1108.563007	85875.166085	34.776039
1109.486737	86022.774244	34.781056
1110.692383	86165.185098	34.786074
1111.667101	86308.891967	34.791092
1112.898021	86455.297075	34.796109
1114.187236	86614.688548	34.801127
1115.265023	86752.659291	34.806144
1116.125474	86907.359550	34.811162
1117.505473	87064.103007	34.816180
1118.796601	87201.404015	34.821197
1120.112227	87340.137468	34.826215
1121.254420	87494.329178	34.831232
1122.961030	87630.472843	34.836250
1123.511428	87780.232920	34.841268
1124.381340	87919.445693	34.846285
1125.440572	88077.588160	34.851303
1126.639520	88234.735680	34.856320
1127.881107	88395.039530	34.861338
1128.742809	88557.928249	34.866356
1129.656579	88705.328659	34.871373
1131.396706	88853.635801	34.876391
1132.234455	89012.459023	34.881408
1133.425054	89157.497514	34.886426
1135.006548	89313.788822	34.891444
1136.015793	89466.390346	34.896461
1137.205403	89612.361682	34.901479
1138.692619	89767.994533	34.906496
1139.753260	89911.762208	34.911514
1140.625519	90083.027787	34.916532
1142.196634	90216.647786	34.921549
1143.761042	90369.780795	34.926567
1144.803900	90514.453329	34.931584
1145.939360	90649.985693	34.936602
1146.908457	90802.021033	34.941620
1147.968811	90946.952939	34.946637
1149.269078	91091.404917	34.951655
1150.354271	91241.002454	34.956672
1151.815795	91373.641274	34.961690
1152.533037	91531.274870	34.966708
1153.862332	91676.573591	34.971725
1154.668878	91823.240355	34.976743
1155.711487	91984.595099	34.981760
1156.656187	92124.606986	34.986778
1157.674389	92274.481487	34.991796
1158.738364	92411.585664	34.996813
1159.708834	92556.725835	35.001831
1160.782267	92716.202426	35.006848
1162.100992	92857.759728	35.011866
1162.708374	93018.451133	35.016884
1163.579013	93171.296391	35.021901
1164.977713	93337.816388	35.026919
1165.739972	93503.211700	35.031936
1167.002878	93669.743112	35.036954
1168.117251	93843.757153	35.041972
1169.798935	93998.123728	35.046989
1171.244429	94153.534694	35.052007
1172.741295	94323.145954	35.057024
1174.257464	94469.755233	35.062042
1175.378878	94626.985875	35.067060
1175.974761	94785.313303	35.072077
1177.727002	94933.033030	35.077095
1178.719047	95100.427828	35.082112
1180.003006	95249.565173	35.087130
1181.236763	95411.369703	35.092148
1182.319932	95570.687916	35.097165
1183.545380	95733.925749	35.102183
1184.626920	95900.717595	35.107200
1185.633618	96049.107213	35.112218
1187.089951	96226.305272	35.117236
1188.160183	96379.191182	35.122253
1189.736726	96532.851661	35.127271
1190.832778	96703.234084	35.132288
1192.066339	96861.771965	35.137306
1193.025879	97031.963456	35.142324
1194.108967	97204.002873	35.147341
1195.495517	97366.454986	35.152359
1196.566856	97533.943683	35.157376
1198.434391	97700.800884	35.162394
1198.778351	97870.406895	35.167412
1200.067227	98035.422592	35.172429
1201.682207	98190.150997	35.177447
1203.067652	98354.407082	35.182464
1204.612289	98503.840633	35.187482
1205.756362	98665.100451	35.192500
1206.961953	98828.932988	35.197517
1208.545461	98976.756401	35.202535
1209.239032	99145.917628	35.207552
1210.762157	99283.907832	35.212570
1212.335534	99453.994369	35.217588
1213.585569	99597.850769	35.222605
1215.534273	99740.369514	35.227623
1217.551200	99857.923905	35.232640
1219.014092	99978.490152	35.237658
1220.428713	100104.430201	35.242676
1221.793161	100221.830764	35.247693
1223.137428	100337.488794	35.252711
1224.031773	100455.085497	35.257728
1225.290684	100567.632540	35.262746
1226.114639	100683.685058	35.267764
1226.547729	100793.023621	35.272781
1227.905962	100904.392255	35.277799
1228.416530	101026.962969	35.282816
1229.679012	101152.825317	35.287834
1230.130014	101293.509954	35.292852
1231.073229	101438.521193	35.297869
1232.287717	101573.701343	35.302887
1232.666411	101734.395471	35.307904
1233.969023	101887.844103	35.312922
1234.759116	102054.049737	35.317940
1235.592734	102233.310236	35.322957
1237.023401	102397.423194	35.327975
1238.181414	102581.564175	35.332992
1238.879849	102762.286627	35.338010
1240.269777	102950.241014	35.343028
1241.556867	103138.529651	35.348045
1243.046259	103315.162891	35.353063
1244.368315	103507.745692	35.358080
1246.006470	103686.079309	35.363098
1247.671402	103864.928927	35.368116
1249.197310	104042.333831	35.373133
1250.729695	104204.975001	35.378151
1251.697360	104377.883109	35.383168
1253.130910	104553.464948	35.388186
1254.367645	104726.187253	35.393204
1256.304123	104879.472252	35.398221
1258.030020	105035.835754	35.403239
1259.426945	105200.454451	35.408256
1260.569932	105353.564867	35.413274
1261.803695	105507.263056	35.418292
1262.917004	105667.424026	35.423309
1264.201473	105823.964112	35.428327
1265.146631	106000.032923	35.433344
1266.089268	106173.711112	35.438362
1267.332779	106343.209946	35.443380
1268.403793	106512.161459	35.448397
1269.625292	106683.318040	35.453415
1270.516065	106874.661097	35.458432
1271.960446	107049.721508	35.463450
1273.146998	107228.463427	35.468468
1273.977233	107419.491296	35.473485
1275.795899	107596.192380	35.478503
1277.081971	107781.618885	35.483520
1278.322678	107974.826436	35.488538
1280.027595	108141.663154	35.493556
1281.299649	108322.886977	35.498573
1282.864773	108496.261324	35.503591
1283.689620	108683.736478	35.508608
1285.147863	108864.162520	35.513626
1286.863847	109031.174460	35.518644
1288.169892	109200.828872	35.523661
1289.298099	109379.855357	35.528679
1290.701644	109554.275636	35.533696
1292.350525	109709.200401	35.538714
1294.291307	109861.206004	35.543732
1295.349329	109995.445705	35.548749
1296.751316	110144.949798	35.553767
1297.407965	110298.054738	35.558784
1298.672920	110451.728578	35.563802
1300.345958	110595.723222	35.568820
1301.062360	110755.404705	35.573837
1301.909431	110908.780668	35.578855
1303.345890	111078.977997	35.583872
1304.570776	111242.424180	35.588890
1305.778621	111423.617744	35.593908
1307.029266	111586.656962	35.598925
1309.041036	111726.666914	35.603943
1310.028750	111915.349809	35.608960
1311.080418	112064.402075	35.613978
1312.662041	112242.598558	35.618996
1313.676304	112419.107631	35.624013
1314.871163	112589.619568	35.629031
1316.174731	112778.417034	35.634048
1317.523987	112952.781204	35.639066
1318.580132	113136.227015	35.644084
1319.418023	113316.151002	35.649101
1320.863948	113505.925227	35.654119
1322.212166	113714.930376	35.659136
1323.217571	113903.118941	35.664154
1324.747105	114103.836739	35.669172
1325.890127	114306.998000	35.674189
1327.878511	114483.518657	35.679207
1329.658327	114674.837672	35.684224
1330.815867	114857.317546	35.689242
1332.088697	115045.643032	35.694260
1332.998565	115251.109120	35.699277
1334.596050	115433.713138	35.704295
1335.877108	115640.756825	35.709312
1337.312927	115825.598959	35.714330
1339.289851	116016.023001	35.719348
1340.890019	116195.928549	35.724365
1342.604261	116376.703635	35.729383
1343.927561	116550.374870	35.734400
1345.045030	116725.922475	35.739418
1346.128778	116909.625391	35.744436
1347.539564	117103.319614	35.749453
1349.086514	117292.428507	35.754471
1350.006526	117482.727487	35.759488
1351.107670	117663.799008	35.764506
1352.588306	117856.335395	35.769524
1353.514480	118055.394515	35.774541
1354.907799	118260.744495	35.779559
1356.062516	118454.096948	35.784576
1357.349421	118652.007876	35.789594
1358.750015	118857.608361	35.794612
1359.547185	119068.543030	35.799629
1361.155022	119275.209323	35.804647
1362.115612	119484.487676	35.809664
1363.656326	119698.893289	35.814682
1365.856582	119878.444086	35.819700
1367.662748	120051.840375	35.824717
1369.597915	120224.077477	35.829735
1371.280276	120382.779146	35.834752
1372.625739	120547.627154	35.839770
1374.225063	120700.201437	35.844788
1375.468451	120864.092441	35.849805
1377.053568	121020.812324	35.854823
1378.493337	121182.343700	35.859840
1379.487263	121351.913410	35.864858
1380.319618	121509.756382	35.869876
1381.695203	121693.250230	35.874893
1382.976657	121870.566837	35.879911
1383.994517	122059.971564	35.884928
1385.455884	122246.191379	35.889946
1386.798095	122425.541213	35.894964
1387.578523	122628.514830	35.899981
1389.077737	122814.745263	35.904999
1390.467528	123007.378102	35.910016
1391.470813	123220.833670	35.915034
1392.872072	123416.684845	35.920052
1394.173565	123626.093688	35.925069
1395.370384	123834.697472	35.930087
1396.959140	124042.961920	35.935104
1398.549175	124251.810440	35.940122
1400.252371	124458.628571	35.945140
1401.013949	124677.226131	35.950157
1402.910476	124879.520005	35.955175
1404.513247	125097.214585	35.960192
1405.585511	125313.462482	35.965210
1407.442353	125522.430397	35.970228
1408.539937	125735.232114	35.975245
1409.930239	125952.967297	35.980263
1411.678240	126157.536417	35.985280
1413.000163	126368.065246	35.990298
1414.647023	126577.707983	35.995316
1415.669254	126803.261095	36.000333
1417.151711	127014.782802	36.005351
1418.780771	127229.057148	36.010368
1420.097801	127450.856968	36.015386
1422.239128	127653.297137	36.020404
1424.189417	127849.371623	36.025421
1425.950822	128048.264573	36.030439
1427.417012	128227.937012	36.035456
1428.926238	128429.013747	36.040474
1430.526092	128616.141949	36.045492
1431.407981	128808.491021	36.050509
1432.733600	129001.290333	36.055527
1433.995651	129211.939000	36.060544
1435.086401	129418.651052	36.065562
1436.450203	129620.937709	36.070580
1437.597543	129831.647271	36.075597
1439.322808	130040.112791	36.080615
1440.889121	130248.364395	36.085632
1442.272317	130442.545437	36.090650
1443.859825	130626.838387	36.095668
1445.226089	130833.643756	36.100685
1446.434972	131011.664523	36.105703
1447.676919	131198.169970	36.110720
1449.091103	131402.209844	36.115738
1450.522066	131593.312393	36.120756
1451.668698	131802.186930	36.125773
1453.098512	132003.175128	36.130791
1454.155268	132213.067905	36.135808
1455.472579	132420.703501	36.140826
1456.742362	132640.562529	36.145844
1457.800138	132865.157726	36.150861
1459.223591	133094.587474	36.155879
1460.594265	133329.868685	36.160896
1461.679997	133565.121067	36.165914
1463.160220	133810.791626	36.170932
1464.530794	134053.770072	36.175949
1465.864421	134297.922182	36.180967
1467.249698	134544.843165	36.185984
1468.840199	134800.489619	36.191002
1470.413176	135040.973234	36.196020
1472.042674	135297.416161	36.201037
1474.383290	135527.023566	36.206055
1476.841005	135754.371250	36.211072
1478.971527	135957.214414	36.216090
1481.051142	136169.317668	36.221108
1482.524538	136387.056500	36.226125
1484.183226	136590.169085	36.231143
1485.523075	136794.068722	36.236160
1487.054008	137007.595786	36.241178
1488.592780	137209.274356	36.246196
1489.791645	137429.307524	36.251213
1491.074319	137645.147021	36.256231
1492.501458	137856.504317	36.261248
1493.476837	138079.302450	36.266266
1494.982004	138298.368262	36.271284
1496.354473	138534.045800	36.276301
1497.455573	138758.362463	36.281319
1499.077393	138991.469355	36.286336
1500.786732	139224.754253	36.291354
1502.377363	139447.845020	36.296372
1503.394575	139675.945875	36.301389
1505.456718	139916.391330	36.306407
1507.116347	140136.624660	36.311424
1508.336874	140374.609350	36.316442
1510.104274	140602.395227	36.321460
1511.579702	140834.424301	36.326477
1513.016597	141062.532287	36.331495
1514.656241	141279.545181	36.336512
1516.227326	141505.100316	36.341530
1518.165774	141736.314908	36.346548
1520.009235	141951.297636	36.351565
1522.162004	142157.702743	36.356583
1523.839940	142355.527880	36.361600
1525.703081	142557.025891	36.366618
1527.289714	142733.054741	36.371636
1528.674596	142909.965863	36.376653
1529.725761	143093.205116	36.381671
1531.400185	143267.828821	36.386688
1532.927781	143456.115249	36.391706
1534.539664	143643.274014	36.396724
1536.174635	143833.510328	36.401741
1537.191824	144009.725620	36.406759
1538.984109	144177.364285	36.411776
1540.722807	144362.643947	36.416794
1542.023539	144542.594497	36.421812
1543.432529	144735.597453	36.426829
1545.054748	144927.249452	36.431847
1546.553501	145110.239326	36.436864
1547.755580	145315.688306	36.441882
1549.112919	145510.985885	36.446900
1550.380768	145716.579141	36.451917
1551.722458	145926.902868	36.456935
1553.481902	146138.378546	36.461952
1554.756472	146364.408967	36.466970
1555.814416	146579.497672	36.471988
1557.373481	146809.098826	36.477005
1558.673781	147037.360995	36.482023
1560.651248	147264.705924	36.487040
1561.597605	147503.663346	36.492058
1562.712312	147738.843466	36.497076
1564.176311	147988.535604	36.502093
1565.619119	148241.681196	36.507111
1567.019573	148477.962258	36.512128
1568.516341	148754.784161	36.517146
1570.616815	149003.647773	36.522164
1572.176438	149255.768562	36.527181
1574.306680	149500.156125	36.532199
1576.111024	149755.094353	36.537216
1577.459232	150003.996369	36.542234
1579.116557	150251.025575	36.547252
1580.569206	150502.006625	36.552269
1581.620420	150763.816979	36.557287
1583.547097	151017.541187	36.562304
1585.006744	151287.937296	36.567322
1586.768445	151536.633096	36.572340
1588.251171	151796.443317	36.577357
1590.190833	152062.458850	36.582375
1592.476804	152295.888233	36.587392
1594.335843	152546.325782	36.592410
1596.598450	152771.609817	36.597428
1598.526104	153001.753860	36.602445
1599.904177	153231.365507	36.607463
1601.881939	153454.898974	36.612480
1603.343030	153686.022024	36.617498
1604.875298	153901.641376	36.622516
1606.615500	154134.067160	36.627533
1608.378815	154359.580616	36.632551
1609.923008	154582.176064	36.637568
1610.955210	154805.209315	36.642586
1612.557359	155023.005582	36.647604
1614.118487	155233.747168	36.652621
1614.968393	155451.095056	36.657639
1616.577976	155671.430233	36.662656
1617.704020	155901.455015	36.667674
1618.944921	156141.492994	36.672692
1620.142554	156380.360268	36.677709
1621.154586	156634.094512	36.682727
1622.998655	156875.436623	36.687744
1624.011590	157137.822378	36.692762
1625.658372	157418.014298	36.697780
1627.562763	157682.849404	36.702797
1628.783735	157948.251567	36.707815
1630.360577	158219.724043	36.712832
1631.681644	158511.313086	36.717850
1633.614298	158786.499661	36.722868
1635.019438	159080.527499	36.727885
1636.747022	159368.292788	36.732903
1638.574844	159643.971901	36.737920
1640.072743	159948.530373	36.742938
1641.762453	160240.759924	36.747956
1643.616791	160523.796920	36.752973
1645.050971	160833.280846	36.757991
1646.878869	161120.892179	36.763008
1648.601241	161407.457291	36.768026
1650.582205	161698.460368	36.773044
1652.576340	161990.148533	36.778061
1654.224300	162286.003064	36.783079
1656.358351	162574.820211	36.788096
1657.627027	162867.619852	36.793114
1659.289679	163163.162113	36.798132
1661.062285	163443.774524	36.803149
1662.791887	163743.407319	36.808167
1664.719258	164031.723426	36.813184
1666.463660	164317.749865	36.818202
1668.050412	164601.178165	36.823220
1669.758543	164886.694752	36.828237
1671.212959	165179.115444	36.833255
1673.294930	165458.679353	36.838272
1674.856896	165764.823587	36.843290
1676.210802	166047.995452	36.848308
1678.675519	166321.302777	36.853325
1680.762230	166605.110799	36.858343
1682.919677	166876.035668	36.863360
1684.662761	167154.473717	36.868378
1686.769851	167430.027477	36.873396
1688.309117	167685.328154	36.878413
1690.302176	167945.885823	36.883431
1692.385757	168194.165238	36.888448
1694.114305	168450.519126	36.893466
1695.516093	168707.040769	36.898484
1697.593648	168962.086889	36.903501
1699.078088	169213.905518	36.908519
1701.056212	169459.279699	36.913536
1702.714512	169705.530723	36.918554
1704.163067	169939.410870	36.923572
1705.720980	170166.171524	36.928589
1706.969806	170394.986794	36.933607
1708.635358	170621.009949	36.938624
1710.086350	170866.286403	36.943642
1711.875988	171099.751451	36.948660
1713.607498	171343.920781	36.953677
1716.306370	171550.097684	36.958695
1718.702766	171775.795769	36.963712
1720.154896	172002.672593	36.968730
1722.071557	172221.814888	36.973748
1723.496811	172444.524955	36.978765
1725.044854	172672.874580	36.983783
1727.087169	172893.408720	36.988800
1728.490480	173113.867930	36.993818
1730.456635	173339.998376	36.998836
1732.202446	173574.753474	37.003853
1733.821698	173804.011604	37.008871
1735.525500	174031.938253	37.013888
1736.753334	174272.424953	37.018906
1737.928547	174522.106279	37.023924
1739.633687	174771.819171	37.028941
1740.879136	175037.502652	37.033959
1742.239126	175293.248825	37.038976
1743.741234	175557.841941	37.043994
1745.073125	175838.728081	37.049012
1746.959171	176121.075928	37.054029
1748.437216	176407.233092	37.059047
1750.068332	176696.273227	37.064064
1751.691081	176990.531054	37.069082
1753.575646	177282.148527	37.074100
1755.964628	177558.247632	37.079117
1757.606784	177858.192321	37.084135
1759.735305	178137.508393	37.089152
1761.932228	178425.645911	37.094170
1763.371653	178709.401573	37.099188
1765.781778	178984.973754	37.104205
1767.080257	179266.281411	37.109223
1769.010943	179538.964356	37.114240
1770.923500	179827.296041	37.119258
1772.465675	180097.303626	37.124276
1774.360934	180379.450030	37.129293
1776.593269	180671.162342	37.134311
1778.151682	180946.653899	37.139328
1779.906349	181228.980392	37.144346
1781.274142	181521.673067	37.149364
1783.333333	181808.598887	37.154381
1785.009991	182101.182942	37.159399
1786.412406	182400.220217	37.164416
1788.147275	182697.113096	37.169434
1789.248892	183000.376741	37.174452
1791.794895	183290.077154	37.179469
1794.301084	183588.959871	37.184487
1796.306413	183872.253143	37.189504
1798.475204	184154.659388	37.194522
1799.705371	184430.706852	37.199540
1801.415007	184688.039366	37.204557
1802.687307	184949.021151	37.209575
1804.182866	185229.688316	37.214592
1806.013083	185506.814470	37.219610
1807.623985	185785.195310	37.224628
1809.479931	186058.399632	37.229645
1811.303596	186336.204371	37.234663
1813.151164	186625.935378	37.239680
1815.142258	186898.780581	37.244698
1816.741284	187187.843908	37.249716
1818.854167	187466.167838	37.254733
1820.514774	187756.963432	37.259751
1822.931801	188036.879486	37.264768
1824.505054	188330.788886	37.269786
1826.182218	188612.234405	37.274804
1828.013335	188895.370356	37.279821
1829.389691	189197.184409	37.284839
1831.855401	189480.451522	37.289856
1834.043340	189782.280027	37.294874
1835.546642	190061.807306	37.299892
1837.652654	190357.903524	37.304909
1839.695820	190638.680969	37.309927
1841.840663	190924.786774	37.314944
1843.473441	191225.735175	37.319962
1845.086215	191513.286812	37.324980
1847.090330	191809.052645	37.329997
1849.140622	192104.889066	37.335015
1850.428109	192400.505665	37.340032
1852.390000	192693.516770	37.345050
1854.310065	192998.707343	37.350068
1855.930335	193296.370510	37.355085
1857.652936	193603.372912	37.360103
1859.455399	193910.021828	37.365120
1861.438529	194219.194968	37.370138
1863.094663	194538.283449	37.375156
1865.551397	194833.665259	37.380173
1867.056929	195149.164253	37.385191
1868.968793	195457.759658	37.390208
1870.802960	195773.502224	37.395226
1872.720854	196083.052306	37.400244
1874.843529	196391.746726	37.405261
1876.533083	196708.609445	37.410279
1878.244596	197029.113323	37.415296
1880.452285	197335.400920	37.420314
1882.460852	197657.181481	37.425332
1884.491943	197966.762749	37.430349
1885.814790	198286.904352	37.435367
1888.629003	198578.886954	37.440384
1891.131310	198872.240705	37.445402
1893.072191	199172.450501	37.450420
1895.278148	199463.011264	37.455437
1896.852396	199774.985547	37.460455
1898.870864	200060.920881	37.465472
1900.579106	200346.856166	37.470490
1901.776533	200630.386116	37.475508
1903.421863	200907.309350	37.480525
1904.901967	201192.053949	37.485543
1906.586118	201478.988979	37.490560
1908.692391	201772.167185	37.495578
1910.146184	202077.496719	37.500596
1911.864361	202374.255782	37.505613
1914.022326	202678.651716	37.510631
1915.947451	202982.032641	37.515648
1918.065175	203280.611707	37.520666
1919.365506	203594.186672	37.525684
1921.440864	203910.153763	37.530701
1923.629108	204218.945191	37.535719
1925.234836	204540.067878	37.540736
1927.352385	204850.409862	37.545754
1929.231214	205168.611060	37.550772
1931.243382	205485.536072	37.555789
1932.570722	205823.441117	37.560807
1934.118577	206162.404810	37.565824
1935.820167	206492.320174	37.570842
1937.376865	206855.469565	37.575860
1939.255671	207198.334610	37.580877
1941.355283	207563.115870	37.585895
1943.541271	207920.268668	37.590912
1945.460531	208271.397680	37.595930
1947.585025	208641.792562	37.600948
1949.550396	208988.817825	37.605965
1951.745645	209351.550552	37.610983
1953.624450	209718.525020	37.616000
1955.382206	210075.085272	37.621018
1957.075339	210441.420534	37.626036
1959.282319	210822.238058	37.631053
1961.294569	211182.331527	37.636071
1963.090994	211552.401911	37.641088
1965.437478	211932.784882	37.646106
1967.222991	212304.473613	37.651124
1969.471003	212672.815530	37.656141
1971.443298	213049.303228	37.661159
1973.417585	213420.320774	37.666176
1975.687678	213787.281487	37.671194
1977.648065	214158.825848	37.676212
1979.670592	214530.717876	37.681229
1982.187325	214899.461021	37.686247
1984.211617	215268.170014	37.691264
1986.639941	215620.882909	37.696282
1988.783690	215973.223764	37.701300
1990.777313	216322.885857	37.706317
1993.113058	216681.573450	37.711335
1995.302600	217038.521224	37.716352
1997.395712	217380.237355	37.721370
1998.890168	217741.361864	37.726388
2001.120275	218080.799563	37.731405
2003.155673	218433.791916	37.736423
2004.842703	218784.149495	37.741440
2006.852829	219123.601546	37.746458
2008.898086	219464.306588	37.751476
2011.029793	219781.687578	37.756493
2012.912562	220104.670767	37.761511
2014.619442	220428.292713	37.766528
2016.533796	220781.086854	37.771546
2018.159734	221144.213226	37.776564
2020.304863	221476.543945	37.781581
2022.247149	221812.184216	37.786599
2024.506190	222154.733911	37.791616
2026.441230	222482.683530	37.796634
2028.510627	222822.980667	37.801652
2031.134782	223160.016836	37.806669
2032.977756	223498.092600	37.811687
2034.712070	223847.538829	37.816704
2036.852238	224184.071980	37.821722
2038.864114	224534.823100	37.826740
2040.827977	224873.266343	37.831757
2043.217373	225215.325878	37.836775
2045.376883	225552.191701	37.841792
2047.837869	225898.560011	37.846810
2049.862463	226244.084708	37.851828
2051.842777	226575.395865	37.856845
2054.079591	226918.654747	37.861863
2055.840662	227271.209426	37.866880
2058.014213	227598.405010	37.871898
2060.116305	227960.076574	37.876916
2062.205407	228306.437365	37.881933
2064.347185	228650.022880	37.886951
2066.615551	228999.024607	37.891968
2068.752330	229342.791345	37.896986
2070.641620	229686.674836	37.902004
2073.147900	230031.528431	37.907021
2075.060314	230389.303238	37.912039
2076.702330	230745.573063	37.917056
2078.521373	231092.799992	37.922074
2080.178414	231455.800494	37.927092
2082.264292	231822.594821	37.932109
2084.173465	232203.031873	37.937127
2085.962936	232583.971966	37.942144
2087.601178	232958.714984	37.947162
2089.566203	233358.577235	37.952180
2091.546016	233742.971154	37.957197
2093.610093	234143.100201	37.962215
2095.304275	234555.328401	37.967232
2097.656953	234944.620425	37.972250
2099.419833	235361.158706	37.977268
2101.297404	235774.251603	37.982285
2103.463652	236181.991940	37.987303
2105.741314	236606.301720	37.992320
2108.605881	236997.298011	37.997338
2111.379525	237386.532176	38.002356
2113.908449	237779.743419	38.007373
2116.623217	238164.443170	38.012391
2118.798228	238545.546921	38.017408
2121.502622	238904.800559	38.022426
2123.564455	239255.267364	38.027444
2125.410192	239603.839119	38.032461
2127.460529	239940.517759	38.037479
2129.218565	240287.429051	38.042496
2131.243544	240641.334782	38.047514
2133.209728	240997.333669	38.052532
2135.197800	241351.526712	38.057549
2136.982173	241703.797262	38.062567
2138.764328	242070.115470	38.067584
2140.977290	242439.414441	38.072602
2142.769321	242817.163354	38.077620
2144.835716	243212.624754	38.082637
2147.035688	243582.360840	38.087655
2148.666322	243973.067527	38.092672
2150.810057	244366.742045	38.097690
2152.555805	244769.752084	38.102708
2154.900253	245176.961075	38.107725
2156.955374	245578.552739	38.112743
2159.401635	245995.730484	38.117760
2162.026131	246390.960086	38.122778
2164.252529	246795.042666	38.127796
2166.436494	247203.349666	38.132813
2168.708678	247598.943166	38.137831
2170.691167	248013.228177	38.142848
2172.731619	248424.304526	38.147866
2175.091762	248847.168305	38.152884
2176.923907	249260.769183	38.157901
2179.456125	249677.994111	38.162919
2181.559830	250083.044465	38.167936
2184.366437	250506.273524	38.172954
2186.371413	250928.233656	38.177972
2188.744713	251342.846078	38.182989
2190.941212	251754.769503	38.188007
2192.969362	252172.486793	38.193024
2195.544728	252588.746540	38.198042
2197.805143	252996.115640	38.203060
2200.366963	253412.379336	38.208077
2203.160631	253801.985719	38.213095
2205.142684	254210.290560	38.218112
2207.497609	254603.803796	38.223130
2209.724018	255018.549056	38.228148
2212.077678	255424.765168	38.233165
2214.745652	255811.600994	38.238183
2217.249126	256207.151207	38.243200
2219.870992	256583.809313	38.248218
2222.503459	256968.925384	38.253236
2224.626700	257353.665585	38.258253
2227.005897	257719.745722	38.263271
2228.612887	258107.871305	38.268288
2230.962882	258486.353671	38.273306
2233.566981	258861.544753	38.278324
2235.906840	259238.607261	38.283341
2238.747801	259599.129848	38.288359
2240.818383	259969.453519	38.293376
2242.648534	260319.315716	38.298394
2244.617587	260671.849007	38.303412
2246.353369	261030.033734	38.308429
2248.450935	261377.847931	38.313447
2249.993401	261731.313767	38.318464
2251.869547	262090.671371	38.323482
2254.068851	262459.351822	38.328500
2255.929864	262844.242624	38.333517
2258.027936	263221.627755	38.338535
2259.970877	263620.376446	38.343552
2261.917193	264015.314550	38.348570
2263.769176	264421.597792	38.353588
2265.646585	264834.533023	38.358605
2268.073459	265247.432332	38.363623
2269.650349	265679.519177	38.368640
2272.303749	266098.480091	38.373658
2274.874548	266529.216148	38.378676
2276.921708	266966.691231	38.383693
2278.909362	267397.215591	38.388711
2281.146895	267834.102272	38.393728
2283.509626	268297.642876	38.398746
2285.443960	268747.686336	38.403764
2287.702847	269208.830677	38.408781
2290.285201	269648.890018	38.413799
2292.639771	270114.414459	38.418816
2295.009431	270578.463329	38.423834
2297.519859	271031.185567	38.428852
2299.928757	271490.478137	38.433869
2302.792340	271941.849112	38.438887
2304.970003	272407.427837	38.443904
2307.640181	272869.854763	38.448922
2309.844315	273332.457257	38.453940
2311.865550	273793.208941	38.458957
2314.333488	274249.393424	38.463975
2316.584799	274724.105935	38.468992
2318.855319	275189.847967	38.474010
2321.586048	275649.420172	38.479028
2323.627421	276130.135606	38.484045
2325.829477	276598.225372	38.489063
2328.041071	277075.128475	38.494080
2330.697408	277543.628605	38.499098
2333.062512	278022.005829	38.504116
2335.737753	278494.643323	38.509133
2338.277686	278971.061729	38.514151
2340.830862	279434.395055	38.519168
2342.775534	279903.464104	38.524186
2345.328299	280368.194100	38.529204
2347.726081	280851.441925	38.534221
2350.528408	281305.132060	38.539239
2353.549124	281760.463835	38.544256
2356.518361	282201.069522	38.549274
2359.431767	282630.404662	38.554292
2362.326566	283064.823008	38.559309
2365.891100	283457.524429	38.564327
2368.482869	283863.259082	38.569344
2370.883070	284251.317751	38.574362
2373.451638	284613.946285	38.579380
2375.279883	284989.850614	38.584397
2377.411836	285351.048883	38.589415
2379.162283	285715.685867	38.594432
2381.440459	286094.464495	38.599450
2383.115496	286465.539601	38.604468
2384.827938	286860.283884	38.609485
2386.749353	287257.153806	38.614503
2388.725420	287674.159024	38.619520
2390.673141	288095.893084	38.624538
2393.689618	288499.522780	38.629556
2395.489247	288930.551113	38.634573
2398.107550	289343.463905	38.639591
2400.026625	289784.988676	38.644608
2402.201969	290220.400861	38.649626
2404.818299	290666.640111	38.654644
2406.545826	291119.954319	38.659661
2408.979267	291563.579059	38.664679
2411.478449	292028.149545	38.669696
2413.834910	292495.688385	38.674714
2416.205955	292951.869098	38.679732
2418.370708	293428.250950	38.684749
2420.978988	293900.395477	38.689767
2423.924760	294368.344892	38.694784
2426.656732	294839.019731	38.699802
2429.166998	295300.533055	38.704820
2431.365454	295784.575436	38.709837
2433.531556	296253.685389	38.714855
2435.970456	296735.680454	38.719872
2438.398148	297227.201676	38.724890
2440.795607	297717.532447	38.729908
2443.403198	298198.988768	38.734925
2445.793326	298675.474085	38.739943
2448.508423	299171.211663	38.744960
2450.900473	299670.047101	38.749978
2453.623785	300162.300353	38.754996
2455.443976	300657.108303	38.760013
2457.809301	301156.476688	38.765031
2460.162666	301665.878744	38.770048
2462.347451	302173.400697	38.775066
2464.701921	302685.034340	38.780084
2466.749308	303214.419176	38.785101
2469.173907	303740.465553	38.790119
2471.492117	304274.604179	38.795136
2473.925041	304802.626405	38.800154
2477.026164	305336.611350	38.805172
2479.446787	305871.514766	38.810189
2482.143000	306399.539641	38.815207
2485.524950	306922.729239	38.820224
2488.073943	307435.431445	38.825242
2490.806524	307945.689433	38.830260
2493.177356	308464.790909	38.835277
2495.930027	308978.063898	38.840295
2498.454945	309486.138427	38.845312
2501.081315	309991.908701	38.850330
2503.750745	310464.549198	38.855348
2505.804271	310953.032816	38.860365
2508.213851	311428.326533	38.865383
2511.339455	311895.148467	38.870400
2513.502643	312368.394408	38.875418
2515.994169	312839.706722	38.880436
2518.243108	313316.922460	38.885453
2520.709720	313803.524382	38.890471
2522.818671	314287.615438	38.895488
2525.124523	314789.959763	38.900506
2527.409363	315278.361318	38.905524
2529.499205	315797.243611	38.910541
2532.016211	316303.940683	38.915559
2534.819523	316818.463051	38.920576
2537.188369	317344.429627	38.925594
2539.497911	317854.173685	38.930612
2541.981283	318394.567410	38.935629
2544.628635	318924.646131	38.940647
2547.180173	319459.283024	38.945664
2549.616521	320000.817555	38.950682
2552.374647	320529.777225	38.955700
2554.534527	321080.796541	38.960717
2557.059493	321623.983226	38.965735
2559.849339	322172.991052	38.970752
2562.409448	322735.974184	38.975770
2564.675016	323289.857681	38.980788
2567.388580	323853.570854	38.985805
2570.338864	324404.875015	38.990823
2573.147980	324967.879684	38.995840
2575.259425	325530.051315	39.000858
2578.348726	326083.378954	39.005876
2580.681089	326654.649804	39.010893
2583.582360	327213.484525	39.015911
2586.161121	327779.781469	39.020928
2588.987096	328348.599863	39.025946
2591.995487	328901.894663	39.030964
2594.650115	329472.280717	39.035981
2597.585310	330022.328339	39.040999
2600.249628	330575.081053	39.046016
2602.871145	331138.730063	39.051034
2606.020179	331677.405808	39.056052
2608.514426	332237.384293	39.061069
2611.278425	332772.075208	39.066087
2614.425962	333315.233156	39.071104
2617.058383	333847.752861	39.076122
2619.728828	334383.080923	39.081140
2622.555234	334918.507014	39.086157
2625.364667	335453.982309	39.091175
2628.237443	335971.516839	39.096192
2630.716339	336515.237391	39.101210
2633.504923	337038.591473	39.106228
2635.977210	337562.321518	39.111245
2638.475829	338087.718920	39.116263
2641.290427	338618.444735	39.121280
2643.683423	339139.356058	39.126298
2645.779787	339642.105356	39.131316
2648.003133	340159.328108	39.136333
2650.659545	340650.961321	39.141351
2653.224637	341152.176890	39.146368
2655.478541	341671.717887	39.151386
2657.708912	342179.833081	39.156404
2660.294516	342701.750001	39.161421
2662.800440	343231.316931	39.166439
2666.328243	343746.042789	39.171456
2668.755544	344281.756704	39.176474
2671.594506	344796.760122	39.181492
2673.789822	345337.070851	39.186509
2676.243220	345872.461227	39.191527
2678.909019	346417.460055	39.196544
2681.069869	346974.363910	39.201562
2684.114979	347524.547030	39.206580
2686.820532	348085.034604	39.211597
2689.262886	348646.370527	39.216615
2692.029102	349208.817157	39.221632
2694.450283	349779.131390	39.226650
2697.688068	350344.766283	39.231668
2700.038254	350924.726043	39.236685
2702.754280	351503.225370	39.241703
2705.457575	352075.323463	39.246720
2707.670208	352675.897994	39.251738
2710.630951	353270.026501	39.256756
2713.189630	353867.181723	39.261773
2715.595915	354475.827392	39.266791
2718.295589	355073.986866	39.271808
2720.946066	355682.630112	39.276826
2723.517298	356299.477030	39.281844
2726.853444	356916.652030	39.286861
2729.549924	357529.478782	39.291879
2733.274866	358128.327457	39.296896
2736.476705	358719.180368	39.301914
2739.929843	359308.082679	39.306932
2742.940188	359898.088468	39.311949
2745.502754	360484.756891	39.316967
2748.366065	361076.319489	39.321984
2750.900501	361657.977899	39.327002
2753.589219	362236.838274	39.332020
2756.454664	362843.707185	39.337037
2758.917013	363437.967978	39.342055
2761.743178	364024.016993	39.347072
2764.301088	364632.205126	39.352090
2766.809506	365225.496221	39.357108
2769.377874	365833.108127	39.362125
2771.987365	366447.709251	39.367143
2774.443701	367053.469648	39.372160
2777.450784	367673.649677	39.377178
2780.656263	368272.093101	39.382196
2783.738888	368886.280527	39.387213
2786.574681	369497.021871	39.392231
2789.690388	370097.814000	39.397248
2792.564662	370693.256476	39.402266
2795.098354	371266.161545	39.407284
2798.239117	371810.442574	39.412301
2800.817363	372365.741513	39.417319
2803.790992	372922.442056	39.422336
2806.451498	373481.671192	39.427354
2809.798993	374011.478813	39.432372
2813.017221	374566.088530	39.437389
2815.853950	375110.374034	39.442407
2818.720614	375647.797184	39.447424
2821.182976	376211.916733	39.452442
2823.981567	376753.851851	39.457460
2826.530073	377310.356362	39.462477
2829.045877	377878.097100	39.467495
2832.418364	378428.239719	39.472512
2835.136171	378988.473716	39.477530
2837.995542	379557.150424	39.482548
2840.637117	380123.544709	39.487565
2843.385549	380692.425174	39.492583
2846.634775	381263.095102	39.497600
2849.428334	381845.649785	39.502618
2851.855808	382429.597897	39.507636
2854.290454	383013.459708	39.512653
2856.942680	383625.332925	39.517671
2859.537305	384220.057961	39.522688
2861.998846	384835.188222	39.527706
2864.841997	385448.928812	39.532724
2867.541003	386078.433252	39.537741
2870.074042	386699.456125	39.542759
2873.309357	387329.437326	39.547776
2875.608207	387972.389476	39.552794
2878.424857	388625.519978	39.557812
2881.320178	389277.307197	39.562829
2884.130947	389937.668045	39.567847
2886.689877	390589.281364	39.572864
2889.473273	391276.199900	39.577882
2892.470302	391944.329817	39.582900
2895.286496	392619.550811	39.587917
2898.111843	393299.271032	39.592935
2901.489643	393977.140523	39.597952
2904.199981	394673.892587	39.602970
2907.328837	395344.394865	39.607988
2910.662542	396029.634579	39.613005
2913.409418	396708.512514	39.618023
2916.755874	397384.137497	39.623040
2919.627959	398070.042061	39.628058
2922.451609	398752.593085	39.633076
2925.205355	399447.311101	39.638093
2928.052114	400141.669927	39.643111
2931.270960	400822.289394	39.648128
2934.800816	401496.709791	39.653146
2937.763564	402183.248102	39.658164
2940.826960	402861.034600	39.663181
2943.578680	403557.590512	39.668199
2946.616448	404239.787886	39.673216
2949.398856	404913.366364	39.678234
2952.566309	405561.215441	39.683252
2955.139662	406204.607479	39.688269
2957.736470	406856.651588	39.693287
2960.620926	407498.877283	39.698304
2963.168344	408161.674297	39.703322
2965.909136	408811.955509	39.708340
2968.683366	409473.420545	39.713357
2971.332628	410153.570693	39.718375
2973.882148	410826.776539	39.723392
2976.643644	411532.400153	39.728410
2979.842920	412225.138892	39.733428
2982.750851	412924.623455	39.738445
2985.447993	413632.918643	39.743463
2988.869741	414328.613548	39.748480
2991.917097	415043.433258	39.753498
2994.631246	415765.358118	39.758516
2998.088593	416473.057956	39.763533
3000.933575	417193.608378	39.768551
3004.053421	417916.301522	39.773568
3006.821124	418632.519925	39.778586
3010.381323	419343.755152	39.783604
3013.638922	420074.935172	39.788621
3016.271931	420809.007165	39.793639
3019.451199	421545.658851	39.798656
3022.440403	422282.346249	39.803674
3025.363552	423025.940598	39.808692
3028.756051	423766.425689	39.813709
3031.956794	424504.463608	39.818727
3035.053380	425240.952560	39.823744
3037.995466	425993.531365	39.828762
3040.936950	426732.005080	39.833780
3044.466316	427481.409252	39.838797
3047.248206	428231.189101	39.843815
3050.532139	428967.519898	39.848832
3053.822810	429719.000459	39.853850
3056.836697	430456.826395	39.858868
3059.883777	431223.295835	39.863885
3063.143642	431978.970701	39.868903
3066.793424	432714.022982	39.873920
3069.777017	433458.529572	39.878938
3072.856194	434199.580576	39.883956
3076.237752	434941.676276	39.888973
3079.031040	435698.681998	39.893991
3081.976854	436439.105893	39.899008
3085.437290	437175.603008	39.904026
3088.389472	437915.450311	39.909044
3091.718786	438654.760094	39.914061
3094.806524	439400.111691	39.919079
3098.344838	440137.115815	39.924096
3101.363485	440883.344608	39.929114
3104.309716	441615.790011	39.934132
3107.956795	442349.266873	39.939149
3110.404348	443100.175679	39.944167
3113.427916	443842.261933	39.949184
3116.896857	444562.839908	39.954202
3119.929696	445278.200096	39.959220
3122.925478	445965.296952	39.964237
3125.874299	446675.717693	39.969255
3129.347372	447362.192033	39.974272
3132.368434	448064.966236	39.979290
3135.129156	448751.613629	39.984308
3138.296309	449437.670248	39.989325
3141.314784	450145.342138	39.994343
3144.260432	450856.850316	39.999360
3147.897048	451563.216637	40.004378
3150.845694	452279.892966	40.009396
3154.038919	452986.386499	40.014413
3157.120637	453705.476504	40.019431
3159.820282	454430.018672	40.024448
3162.694105	455165.237675	40.029466
3165.512136	455900.542531	40.034484
3168.749444	456643.700878	40.039501
3171.452031	457397.645588	40.044519
3174.644859	458157.963282	40.049536
3177.698823	458928.446058	40.054554
3180.565128	459703.181156	40.059572
3183.780614	460472.774449	40.064589
3186.852306	461272.615213	40.069607
3189.967360	462064.629166	40.074624
3192.766848	462867.539637	40.079642
3195.316388	463691.400899	40.084660
3198.605795	464511.825568	40.089677
3201.572124	465339.047235	40.094695
3205.033127	466163.275417	40.099712
3208.414602	466999.267889	40.104730
3211.235372	467852.055352	40.109748
3214.469965	468698.775156	40.114765
3217.695393	469568.672977	40.119783
3221.337540	470426.281738	40.124800
3224.817749	471278.166588	40.129818
3227.917789	472154.143875	40.134836
3232.213894	472981.002597	40.139853
3235.765203	473823.820746	40.144871
3238.958186	474668.328801	40.149888
3242.717887	475513.925120	40.154906
3246.163761	476365.753294	40.159924
3249.348204	477199.641324	40.164941
3252.426202	478039.930768	40.169959
3255.719973	478893.443883	40.174976
3259.049405	479730.639486	40.179994
3262.372863	480567.244385	40.185012
3265.896769	481410.655085	40.190029
3269.225720	482251.230024	40.195047
3272.166402	483093.244892	40.200064
3275.574157	483941.314134	40.205082
3278.961452	484784.852033	40.210100
3282.408867	485618.288221	40.215117
3285.269653	486465.978471	40.220135
3288.668910	487299.399194	40.225152
3292.362957	488127.179255	40.230170
3295.828727	488924.243474	40.235188
3299.662599	489688.935292	40.240205
3302.786691	490474.368679	40.245223
3306.533515	491240.526144	40.250240
3310.088890	492003.197020	40.255258
3313.346329	492755.983862	40.260276
3316.690379	493517.918468	40.265293
3319.611809	494295.544676	40.270311
3322.793747	495069.308983	40.275328
3325.911122	495840.576160	40.280346
3328.601234	496635.460719	40.285364
3331.768813	497425.033829	40.290381
3335.006408	498233.748842	40.295399
3338.079678	499033.163061	40.300416
3341.434993	499847.643685	40.305434
3343.867773	500676.621666	40.310452
3347.444459	501498.413305	40.315469
3350.740060	502343.432902	40.320487
3353.754086	503189.011809	40.325504
3356.859295	504049.476794	40.330522
3359.931471	504915.254998	40.335540
3363.570922	505777.922687	40.340557
3366.533661	506664.122783	40.345575
3369.664707	507549.796684	40.350592
3372.813955	508440.569540	40.355610
3375.961865	509339.824386	40.360628
3379.084282	510253.820412	40.365645
3382.282658	511176.736565	40.370663
3385.528082	512116.042843	40.375680
3388.864668	513055.786991	40.380698
3391.663277	514005.855015	40.385716
3395.364844	514946.898601	40.390733
3398.767678	515910.282102	40.395751
3402.058693	516885.531020	40.400768
3405.816860	517857.319857	40.405786
3409.289196	518817.648296	40.410804
3413.163484	519785.169367	40.415821
3416.628046	520753.504775	40.420839
3420.014656	521729.156822	40.425856
3424.118393	522708.670484	40.430874
3427.510255	523677.649499	40.435892
3431.320310	524640.353424	40.440909
3435.052338	525605.129124	40.445927
3438.710894	526569.807694	40.450944
3442.432975	527529.780341	40.455962
3445.879409	528488.982303	40.460980
3449.671387	529436.983383	40.465997
3453.196695	530403.162560	40.471015
3456.524306	531355.707094	40.476032
3460.318372	532299.805273	40.481050
3463.595171	533263.881179	40.486068
3467.247912	534209.648896	40.491085
3470.618131	535176.361737	40.496103
3473.714877	536133.837773	40.501120
3477.259688	537066.956906	40.506125
3480.503114	537974.169767	40.511130
3484.125172	538809.107318	40.516135
3487.124133	539598.096199	40.521140
3489.882185	540318.462329	40.526144
3493.177408	540965.093909	40.531149
3495.844711	541561.257828	40.536154
3498.592822	542085.492130	40.541159
3501.376381	542554.522136	40.546164
3503.450808	542957.465214	40.551168
3505.670122	543313.122761	40.556173
3507.470394	543608.007712	40.561178
3508.920794	543836.862736	40.566183
3511.030333	544039.966129	40.571188
3512.607086	544183.988815	40.576192
3514.290306	544282.158057	40.581197
3515.359505	544340.595658	40.586202
3516.236677	544358.276295	40.591207
3517.475343	544342.634035	40.596212
3518.428918	544292.458499	40.601216
3519.353814	544218.511452	40.606221
3519.678163	544121.791554	40.611226
3520.393009	543995.377370	40.616231
3520.761206	543847.764466	40.621236
3520.924327	543678.828872	40.626240
3521.767981	543499.334028	40.631245
3522.324670	543298.275779	40.636250
3522.362312	543086.998226	40.641255
3522.591479	542858.270361	40.646260
3522.630889	542611.646793	40.651264
3522.798977	542352.730737	40.656269
3522.893002	542113.107846	40.661274
3523.132172	541837.510998	40.666279
3523.385517	541563.270029	40.671284
3523.191574	541280.763957	40.676288
3523.038572	540995.216662	40.681293
3522.887361	540705.371878	40.686298
3522.746446	540411.026049	40.691303
3522.905280	540118.242880	40.696308
3522.779850	539816.611926	40.701312
3522.605085	539511.397557	40.706317
3522.401668	539228.349497	40.711322
3522.934528	538915.285301	40.716327
3522.618385	538607.045172	40.721332
3522.618026	538309.050766	40.726336
3522.252559	537992.776522	40.731341
3521.786926	537680.804158	40.736346
3521.884428	537374.392688	40.741351
3521.551182	537079.709460	40.746356
3521.584686	536772.588954	40.751360
3521.597166	536466.879749	40.756365
3521.069075	536171.856247	40.761370
3521.063607	535861.945740	40.766375
3520.753670	535577.937475	40.771380
3520.509315	535285.579520	40.776384
3520.452601	534986.721003	40.781389
3519.948226	534697.322555	40.786394
3519.901356	534408.604044	40.791399
3519.626117	534127.846805	40.796404
3519.381540	533845.665212	40.801408
3519.104035	533565.807362	40.806413
3518.918090	533290.880548	40.811418
3518.999511	533007.571300	40.816423
3518.642434	532744.583831	40.821428
3518.020167	532477.491281	40.826432
3517.975439	532217.880791	40.831437
3517.609065	531966.450576	40.836442
3517.656167	531697.723226	40.841447
3517.340313	531446.175581	40.846452
3517.141923	531200.263871	40.851456
3517.191892	530947.488345	40.856461
3516.575157	530715.478588	40.861466
3516.592432	530466.893981	40.866471
3516.514916	530224.939314	40.871476
3515.996585	529988.760100	40.876480
3516.115086	529758.994729	40.881485
3515.870569	529531.607665	40.886490
3515.779952	529301.262310	40.891495
3515.696136	529074.247466	40.896500
3515.472462	528844.775461	40.901504
3515.181369	528619.151137	40.906509
3514.556879	528415.406025	40.911514
3514.483099	528204.900961	40.916519
3514.793091	528008.127981	40.921524
3514.301264	527801.574663	40.926528
3514.281257	527587.919794	40.931533
3514.015104	527386.985256	40.936538
3513.850519	527192.298545	40.941543
3513.681878	527005.342140	40.946548
3513.451971	526808.791205	40.951552
3513.606845	526613.339389	40.956557
3513.239935	526429.035490	40.961562
3512.998592	526249.814019	40.966567
3512.780123	526063.208183	40.971572
3512.301669	525891.904285	40.976576
3512.430060	525722.625334	40.981581
3512.270633	525544.545415	40.986586
3512.251068	525370.181477	40.991591
3511.857819	525202.647327	40.996596
3512.298548	525043.066418	41.001600
3512.254547	524871.480745	41.006605
3511.447688	524712.295888	41.011610
3511.385354	524553.901572	41.016615
3511.622724	524393.588177	41.021620
3511.182427	524246.926355	41.026624
3510.999552	524104.063964	41.031629
3510.891329	523953.050610	41.036634
3510.717101	523798.356380	41.041639
3510.645142	523661.841379	41.046644
3510.664646	523527.534845	41.051648
3510.704731	523376.947571	41.056653
3510.544483	523240.392404	41.061658
3510.461641	523095.634970	41.066663
3510.168155	522963.091855	41.071668
3509.978991	522821.836653	41.076672
3509.725002	522701.113722	41.081677
3509.141168	522577.257354	41.086682
3509.690127	522448.368139	41.091687
3509.410829	522332.701522	41.096692
3509.042813	522209.718147	41.101696
3509.524288	522091.755861	41.106701
3508.955623	521979.165558	41.111706
3508.928908	521870.179149	41.116711
3509.202887	521756.493625	41.121716
3508.916262	521648.760074	41.126720
3508.942715	521527.074111	41.131725
3508.659592	521416.254697	41.136730
3508.577132	521307.071103	41.141735
3508.564753	521211.879305	41.146740
3508.358817	521109.993751	41.151744
3508.861702	520999.856150	41.156749
3508.383751	520895.686707	41.161754
3508.620031	520791.555381	41.166759
3508.148497	520688.445270	41.171764
3508.137862	520589.660073	41.176768
3507.884851	520489.345325	41.181773
3507.902304	520401.272576	41.186778
3508.229632	520298.387639	41.191783
3507.800840	520209.474351	41.196788
3507.644552	520120.517510	41.201792
3507.684426	520025.108293	41.206797
3507.262719	519943.220023	41.211802
3507.255080	519857.018968	41.216807
3507.394408	519771.047026	41.221812
3507.400031	519688.533793	41.226816
3507.307400	519608.715326	41.231821
3507.305346	519526.101369	41.236826
3507.205149	519439.356586	41.241831
3507.440413	519358.322196	41.246836
3507.013460	519272.336015	41.251840
3507.132847	519185.504624	41.256845
3506.824018	519109.206587	41.261850
3506.759299	519043.538036	41.266855
3506.934851	518967.365029	41.271860
3506.661843	518889.745711	41.276864
3506.599854	518812.648857	41.281869
3506.412006	518747.099704	41.286874
3506.542429	518675.887567	41.291879
3506.657930	518610.795550	41.296884
3506.372535	518541.165426	41.301888
3506.714183	518469.211131	41.306893
3506.432950	518399.933691	41.311898
3506.231384	518338.682950	41.316903
3506.214728	518279.779244	41.321908
3506.193085	518206.869949	41.326912
3506.039464	518137.975748	41.331917
3505.618375	518090.360491	41.336922
3505.987037	518029.473553	41.341927
3505.758187	517975.001391	41.346932
3505.486547	517930.193663	41.351936
3505.864925	517864.096419	41.356941
3505.909213	517807.659071	41.361946
3505.336987	517746.161319	41.366951
3505.781053	517701.340982	41.371956
3505.848873	517644.444268	41.376960
3505.832806	517590.038336	41.381965
3505.619705	517543.096545	41.386970
3505.512048	517490.171168	41.391975
3505.579584	517429.582441	41.396980
3505.133848	517383.486022	41.401984
3505.791659	517327.759129	41.406989
3505.453918	517282.909523	41.411994
3505.302893	517231.962272	41.416999
3505.133985	517180.208619	41.422004
3505.074246	517145.680923	41.427008
3505.393924	517091.473121	41.432013
3505.052393	517058.709065	41.437018
3505.539422	517006.497227	41.442023
3505.519930	516962.354965	41.447028
3505.262711	516914.407008	41.452032
3505.251376	516867.734816	41.457037
3505.164137	516829.215942	41.462042
3504.956614	516782.068836	41.467047
3505.269391	516738.631985	41.472052
3505.058615	516693.558440	41.477056
3505.412318	516644.552347	41.482061
3504.949722	516613.222463	41.487066
3505.235306	516572.621321	41.492071
3505.069561	516519.246901	41.497076
3505.056420	516481.018920	41.502080
3505.194192	516438.620324	41.507085
3504.958545	516396.988610	41.512090
3505.008886	516343.427764	41.517095
3504.725304	516321.474959	41.522100
3504.589681	516283.973856	41.527104
3504.976084	516232.028335	41.532109
3504.415518	516199.802897	41.537114
3504.913829	516158.711992	41.542119
3504.866548	516127.821251	41.547124
3504.761018	516097.040798	41.552128
3504.857615	516056.468264	41.557133
3504.604149	516016.153241	41.562138
3504.798737	515968.839129	41.567143
3505.118741	515938.547405	41.572148
3504.409087	515906.142676	41.577152
3504.769939	515861.836231	41.582157
3504.851727	515837.043635	41.587162
3504.593349	515793.391158	41.592167
3504.818720	515758.410944	41.597172
3504.602089	515721.578802	41.602176
3504.858340	515685.784412	41.607181
3504.553857	515659.990601	41.612186
3504.756995	515613.988990	41.617191
3504.460069	515583.086122	41.622196
3504.403914	515551.689995	41.627200
3504.718146	515511.435739	41.632205
3504.746951	515483.212092	41.637210
3504.443816	515445.229851	41.642215
3504.409128	515402.552440	41.647220
3504.605583	515387.602659	41.652224
3504.833351	515358.184189	41.657229
3504.539261	515321.717412	41.662234
3504.544248	515292.485755	41.667239
3504.531584	515249.096452	41.672244
3504.381758	515224.238406	41.677248
3504.408162	515184.433435	41.682253
3504.366460	515166.334996	41.687258
3504.128919	515133.601277	41.692263
3504.209078	515106.835499	41.697268
3504.224518	515076.034039	41.702272
3504.299868	515047.043698	41.707277
3504.026227	515033.179367	41.712282
3504.386497	514995.141823	41.717287
3504.251404	514969.522464	41.722292
3504.241243	514942.315534	41.727296
3504.597616	514905.745041	41.732301
3503.909972	514878.999102	41.737306
3504.339097	514857.437459	41.742311
3504.269257	514838.533928	41.747316
3504.319492	514809.547144	41.752320
3504.152620	514779.127970	41.757325
3504.181133	514750.397388	41.762330
3504.246993	514718.980410	41.767335
3504.267689	514699.556668	41.772340
3504.015101	514676.939325	41.777344
3504.355958	514651.193679	41.782349
3503.879852	514632.101252	41.787354
3504.014090	514604.567501	41.792359
3504.176277	514571.466054	41.797364
3503.987169	514552.227025	41.802368
3504.166072	514518.212481	41.807373
3503.829295	514509.010595	41.812378
3503.894636	514472.990905	41.817383
3504.063352	514460.118262	41.822388
3504.040785	514428.562988	41.827392
3504.209446	514409.115523	41.832397
3504.212104	514387.216076	41.837402
3504.042577	514363.674824	41.842407
3504.249565	514333.398052	41.847412
3504.110908	514303.985067	41.852416
3504.372747	514282.550276	41.857421
3504.240239	514259.357056	41.862426
3504.185084	514228.666345	41.867431
3504.141247	514202.070445	41.872436
3503.924080	514167.005115	41.877440
3504.225589	514152.998574	41.882445
3504.254540	514129.627927	41.887450
3504.072947	514105.026117	41.892455
3503.871116	514077.797499	41.897460
3503.886704	514061.357829	41.902464
3504.031998	514032.607558	41.907469
3503.852688	514019.132087	41.912474
3503.892182	513980.738327	41.917479
3504.142026	513972.404386	41.922484
3503.812413	513952.984568	41.927488
3504.305572	513932.372575	41.932493
3503.965873	513905.721811	41.937498
3504.004838	513887.154047	41.942503
3504.086580	513856.086979	41.947508
3503.906737	513835.176619	41.952512
3503.801385	513803.178058	41.957517
3503.696174	513799.502672	41.962522
3503.951266	513765.778023	41.967527
3504.068277	513759.589218	41.972532
3503.918713	513738.775107	41.977536
3504.034284	513707.500107	41.982541
3504.106066	513676.940057	41.987546
3503.765527	513652.514436	41.992551
3503.806861	513633.844862	41.997556
3503.801539	513622.769303	42.002560
3504.076147	513594.351888	42.007565
3503.676412	513589.863182	42.012570
3503.542636	513555.592639	42.017575
3503.829017	513537.238273	42.022580
3503.666778	513524.214908	42.027584
3503.725693	513502.052524	42.032589
3503.751008	513493.703255	42.037594
3503.694745	513469.131282	42.042599
3503.847598	513453.023369	42.047604
3503.874667	513434.406406	42.052608
3504.081130	513413.485043	42.057613
3503.721759	513398.570759	42.062618
3504.009947	513375.259246	42.067623
3503.731687	513352.543014	42.072628
3503.722139	513329.480810	42.077632
3504.035893	513314.358906	42.082637
3503.939441	513290.754019	42.087642
3503.859072	513276.705947	42.092647
3503.763401	513250.015573	42.097652
3503.594164	513240.938245	42.102656
3504.053170	513209.608039	42.107661
3503.743582	513193.775284	42.112666
3503.723879	513178.807120	42.117671
3503.968561	513159.902564	42.122676
3503.573909	513146.763902	42.127680
3503.896997	513106.401313	42.132685
3503.871822	513113.992304	42.137690
3503.723866	513080.279405	42.142695
3503.611352	513061.987567	42.147700
3503.922468	513050.861619	42.152704
3503.950130	513014.541279	42.157709
3503.706693	513002.794832	42.162714
3503.910391	512985.110468	42.167719
3503.883114	512962.910417	42.172724
3503.584517	512937.718433	42.177728
3503.584365	512924.517245	42.182733
3503.697607	512913.574220	42.187738
3503.902952	512890.224550	42.192743
3503.934201	512885.566377	42.197748
3503.643059	512845.907203	42.202752
3504.125079	512823.778215	42.207757
3503.530164	512812.542408	42.212762
3503.681519	512796.484684	42.217767
3503.615912	512779.095570	42.222772
3503.604837	512753.908447	42.227776
3503.889123	512739.043587	42.232781
3503.694329	512730.324085	42.237786
3504.068720	512708.616600	42.242791
3503.629036	512681.271569	42.247796
3503.734986	512665.524381	42.252800
3503.851553	512646.690080	42.257805
3503.836952	512624.942806	42.262810
3503.743480	512613.627612	42.267815
3503.820306	512584.936270	42.272820
3503.624301	512572.979703	42.277824
3503.652971	512563.668406	42.282829
3503.737866	512551.920332	42.287834
3503.962409	512530.236301	42.292839
3503.875344	512498.434693	42.297844
3503.515496	512495.659145	42.302848
3504.056757	512468.108147	42.307853
3503.548121	512453.924753	42.312858
3503.730429	512435.990288	42.317863
3503.712613	512409.286277	42.322868
3504.007528	512405.901415	42.327872
3503.630037	512375.005359	42.332877
3503.510045	512363.289536	42.337882
3503.922910	512346.380749	42.342887
3503.951840	512319.871535	42.347892
3503.623425	512307.834543	42.352896
3504.008262	512285.517884	42.357901
3503.816495	512278.871521	42.362906
3503.686692	512250.313433	42.367911
3503.853904	512234.960816	42.372916
3503.910230	512211.330269	42.377920
3503.938266	512194.735064	42.382925
3503.748966	512173.571223	42.387930
3503.804598	512154.796586	42.392935
3504.032883	512128.710803	42.397940
3503.468992	512112.006742	42.402944
3504.013717	512083.645255	42.407949
3503.770349	512068.306797	42.412954
3503.616794	512055.129176	42.417959
3503.690121	512035.542291	42.422964
3503.718018	512020.110333	42.427968
3503.939592	512004.192507	42.432973
3503.731004	511991.327029	42.437978
3503.566964	511963.279693	42.442983
3503.732937	511943.779225	42.447988
3503.361865	511936.452908	42.452992
3503.318882	511925.685683	42.457997
3503.387289	511902.457458	42.463002
3503.497007	511883.218726	42.468007
3503.595329	511866.662672	42.473012
3503.521981	511858.783435	42.478016
3503.636238	511844.399911	42.483021
3503.244780	511849.570791	42.488026
3503.255706	511828.779536	42.493031
3503.492031	511809.217211	42.498036
3503.220145	511812.042378	42.503040
3503.294699	511803.279825	42.508045
3503.149122	511789.746653	42.513050
3503.084122	511778.729898	42.518055
3503.035501	511761.286467	42.523060
3503.098125	511760.770856	42.528064
3503.395217	511754.401105	42.533069
3503.130150	511763.699868	42.538074
3503.353160	511737.361399	42.543079
3503.413663	511713.425996	42.548084
3503.153344	511724.089784	42.553088
3503.311747	511716.376186	42.558093
3503.222145	511688.417795	42.563098
3503.275463	511671.565163	42.568103
3503.316328	511670.091901	42.573108
3503.300684	511667.362979	42.578112
3503.769205	511644.121745	42.583117
3503.091667	511648.376812	42.588122
3503.284397	511630.186929	42.593127
3503.574355	511623.211251	42.598132
3503.415366	511609.073050	42.603136
3503.542834	511582.597690	42.608141
3503.393419	511576.146691	42.613146
3503.286764	511551.832809	42.618151
3503.333577	511543.883850	42.623156
3503.490655	511552.761919	42.628160
3503.337534	511534.171340	42.633165
3503.324394	511522.893303	42.638170
3503.477938	511508.907957	42.643175
3503.468377	511504.255853	42.648180
3503.011375	511474.938825	42.653184
3503.405157	511452.063230	42.658189
3503.330074	511451.569375	42.663194
3502.998461	511455.162803	42.668199
3503.168962	511453.213775	42.673204
3502.797068	511430.965010	42.678208
3503.231923	511414.658831	42.683213
3503.014837	511422.280914	42.688218
3502.788169	511418.421865	42.693223
3503.268834	511416.727317	42.698228
3503.106610	511418.270607	42.703232
3502.807079	511401.473475	42.708237
3502.955053	511390.220469	42.713242
3502.754127	511386.357345	42.718247
3503.020558	511382.369768	42.723252
3503.033241	511378.574050	42.728256
3503.567269	511374.341840	42.733261
3503.254841	511381.523749	42.738266
3503.415948	511369.712225	42.743271
3503.436787	511349.121153	42.748276
3503.279426	511341.710215	42.753280
3503.633426	511344.234198	42.758285
3503.370226	511323.435065	42.763290
3503.472293	511308.496582	42.768295
3503.326859	511299.819123	42.773300
3503.388978	511271.532557	42.778304
3503.756721	511263.380989	42.783309
3503.470239	511255.029309	42.788314
3503.330379	511236.638647	42.793319
3503.517538	511216.425806	42.798324
3503.081486	511211.486935	42.803329
3503.535303	511208.936665	42.808333
3503.566702	511195.172707	42.813338
3503.771759	511183.354107	42.818343
3503.313866	511178.216338	42.823348
3503.232197	511166.139533	42.828353
3503.438097	511135.604272	42.833357
3503.134402	511143.189582	42.838362
3503.141618	511134.993764	42.843367
3503.505982	511106.912079	42.848372
3503.520644	511095.679949	42.853377
3503.707109	511093.323674	42.858381
3503.358957	511071.880050	42.863386
3503.338530	511058.326513	42.868391
3503.335312	511052.307477	42.873396
3503.436434	511046.727216	42.878401
3503.832655	511024.912956	42.883405
3503.694376	511019.977550	42.888410
3503.233252	510988.029882	42.893415
3503.318502	510977.646473	42.898420
3503.417992	510972.319374	42.903425
3503.508388	510956.674228	42.908429
3503.483123	510938.720402	42.913434
3503.498281	510928.955070	42.918439
3503.365433	510922.450618	42.923444
3503.403370	510899.731694	42.928449
3503.277150	510887.307631	42.933453
3503.493229	510883.833757	42.938458
3503.550241	510868.042047	42.943463
3503.440699	510856.981148	42.948468
3503.502010	510848.624883	42.953473
3503.417391	510829.921533	42.958477
3503.539620	510812.652468	42.963482
3503.774961	510808.214397	42.968487
3503.782164	510792.430490	42.973492
3503.362540	510762.600459	42.978497
3503.695493	510746.916783	42.983501
3503.337896	510745.809937	42.988506
3503.522270	510722.207663	42.993511
3503.538216	510713.150293	42.998516
3503.645581	510701.599731	43.003521
3503.708573	510674.526109	43.008525
3503.213354	510673.946875	43.013530
3503.445827	510658.633105	43.018535
3503.779320	510626.913273	43.023540
3503.190780	510631.710975	43.028545
3503.654580	510618.788768	43.033549
3503.585361	510593.557036	43.038554
3503.525271	510575.102463	43.043559
3503.670338	510553.984924	43.048564
3503.511259	510545.056301	43.053569
3503.614444	510532.545134	43.058573
3503.719621	510533.186262	43.063578
3503.718113	510501.114447	43.068583
3503.644200	510495.359322	43.073588
3503.133392	510475.913549	43.078593
3503.410569	510451.840950	43.083597
3503.552721	510452.577411	43.088602
3503.468211	510442.271093	43.093607
3503.700084	510414.866843	43.098612
3503.359687	510420.991242	43.103617
3503.859245	510396.377543	43.108621
3503.359117	510380.724026	43.113626
3503.236769	510365.921361	43.118631
3503.736637	510350.666227	43.123636
3503.310063	510332.319902	43.128641
3503.285867	510322.256916	43.133645
3503.109166	510326.079034	43.138650
3503.236234	510300.208792	43.143655
3503.205085	510277.854071	43.148660
3503.025418	510280.462563	43.153665
3503.129678	510265.371055	43.158669
3503.160122	510278.418004	43.163674
3503.067226	510255.769487	43.168679
3503.477940	510240.528346	43.173684
3503.064239	510238.823278	43.178689
3503.299961	510237.926149	43.183693
3503.341654	510236.149104	43.188698
3503.140204	510210.887116	43.193703
3503.447871	510192.930471	43.198708
3503.235089	510201.007710	43.203713
3503.375477	510184.443370	43.208717
3503.230573	510167.671164	43.213722
3503.396733	510149.787428	43.218727
3503.629779	510140.897792	43.223732
3503.434302	510136.072346	43.228737
3503.637840	510109.430906	43.233741
3503.388255	510106.688121	43.238746
3503.510146	510092.150144	43.243751
3503.556119	510073.425322	43.248756
3503.201212	510059.367383	43.253761
3503.379808	510062.273402	43.258765
3503.064779	510042.644424	43.263770
3503.085007	510026.149511	43.268775
3503.407246	510016.233944	43.273780
3503.233039	510011.202746	43.278785
3503.307801	510005.929843	43.283789
3503.318161	509985.996428	43.288794
3503.171911	509974.434870	43.293799
3503.507575	509967.957181	43.298804
3503.425470	509963.518476	43.303809
3503.345654	509938.489802	43.308813
3503.343477	509942.942075	43.313818
3503.366399	509939.802071	43.318823
3503.646686	509913.552906	43.323828
3503.076977	509896.796986	43.328833
3503.450020	509886.316837	43.333837
3503.224665	509890.298508	43.338842
3503.105612	509864.162972	43.343847
3503.321601	509848.142836	43.348852
3503.480012	509845.487290	43.353857
3503.392686	509837.862269	43.358861
3503.367709	509830.885048	43.363866
3503.392437	509826.277655	43.368871
3503.457473	509812.911976	43.373876
3503.146965	509802.286866	43.378881
3503.503222	509777.290213	43.383885
3503.228259	509776.220829	43.388890
3503.527189	509777.843147	43.393895
3503.565968	509752.896636	43.398900
3503.133764	509739.913025	43.403905
3503.219363	509728.365245	43.408909
3503.359772	509727.938458	43.413914
3503.402877	509711.338446	43.418919
3503.684111	509699.506779	43.423924
3503.521415	509684.962846	43.428929
3503.344414	509666.728126	43.433933
3503.228585	509660.119321	43.438938
3503.449339	509644.806495	43.443943
3503.640810	509643.106896	43.448948
3503.242877	509616.559751	43.453953
3503.335413	509598.940023	43.458957
3503.440073	509596.242345	43.463962
3503.169289	509586.622618	43.468967
3503.192707	509570.683248	43.473972
3503.055984	509559.271672	43.478977
3503.161734	509543.825163	43.483981
3503.166472	509558.090883	43.488986
3503.019677	509545.770272	43.493991
3503.290318	509518.914947	43.498996
3502.755308	509514.901837	43.504001
3503.292221	509511.680517	43.509005
3503.069538	509516.370113	43.514010
3503.044226	509513.389424	43.519015
3503.148723	509508.718748	43.524020
3503.165473	509490.200266	43.529025
3503.215272	509480.580399	43.534029
3503.297307	509479.505162	43.539034
3503.366193	509474.890695	43.544039
3503.280796	509451.025762	43.549044
3503.275410	509435.293179	43.554049
3503.364219	509430.928502	43.559053
3503.308030	509430.026879	43.564058
3502.999426	509407.006607	43.569063
3503.285185	509393.706895	43.574068
3503.192210	509387.347324	43.579073
3503.145723	509377.135533	43.584077
3502.937419	509384.453593	43.589082
3502.776986	509385.187335	43.594087
3503.103109	509366.215099	43.599092
3503.054905	509350.995110	43.604097
3503.161652	509341.012032	43.609101
3503.313205	509337.649225	43.614106
3503.232345	509326.886341	43.619111
3503.526614	509320.667903	43.624116
3503.332408	509305.673312	43.629121
3503.308227	509303.198314	43.634125
3503.277191	509301.280896	43.639130
3503.241614	509283.731683	43.644135
3503.269447	509255.396600	43.649140
3502.917884	509256.565283	43.654145
3503.167750	509249.139659	43.659149
3503.151357	509252.936678	43.664154
3503.192927	509243.419161	43.669159
3503.211231	509227.935597	43.674164
3503.179242	509217.316692	43.679169
3503.696870	509210.658186	43.684173
3503.039420	509205.096036	43.689178
3503.190004	509179.422745	43.694183
3503.266257	509165.548877	43.699188
3503.181409	509167.484867	43.704193
3503.249908	509175.821677	43.709197
3502.990984	509155.525128	43.714202
3503.063251	509127.081628	43.719207
3503.194226	509122.558435	43.724212
3503.262268	509123.660807	43.729217
3503.228253	509117.696546	43.734221
3502.893349	509118.356693	43.739226
3502.646299	509094.972134	43.744231
3502.995448	509079.790284	43.749236
3502.615770	509086.781417	43.754241
3502.766790	509071.226144	43.759245
3502.987615	509072.607919	43.764250
3503.149877	509075.213141	43.769255
3503.180167	509077.080352	43.774260
3502.491266	509078.909458	43.779265
3503.042345	509073.560985	43.784269
3502.706675	509081.405217	43.789274
3503.207764	509072.219707	43.794279
3503.272599	509049.645843	43.799284
3502.897980	509049.603990	43.804289
3502.985269	509037.397790	43.809293
3502.796350	509043.245780	43.814298
3503.065736	509035.412247	43.819303
3503.462768	509037.727412	43.824308
3502.930770	509023.443651	43.829313
3502.942930	509003.002892	43.834317
3502.883746	509003.467690	43.839322
3502.946592	508996.273882	43.844327
3503.055744	508996.914440	43.849332
3502.705106	508999.853696	43.854337
3503.233900	508998.151311	43.859341
3503.271220	508999.511504	43.864346
3503.298525	508966.268649	43.869351
3503.412486	508964.378867	43.874356
3503.291816	508960.350729	43.879361
3503.349755	508947.592596	43.884365
3502.995213	508930.447575	43.889370
3502.907253	508914.272239	43.894375
3503.154264	508907.049286	43.899380
3503.024041	508911.471474	43.904385
3503.146594	508911.148674	43.909389
3503.508355	508916.808487	43.914394
3503.258559	508889.022596	43.919399
3503.672166	508882.076853	43.924404
3503.215741	508880.428988	43.929409
3503.451290	508853.476984	43.934413
3503.538065	508843.952100	43.939418
3503.306120	508832.555089	43.944423
3503.747089	508819.028033	43.949428
3503.234181	508806.258834	43.954433
3503.522415	508786.988394	43.959437
3503.427213	508784.322177	43.964442
3503.636750	508764.760597	43.969447
3503.565031	508744.585749	43.974452
3503.223576	508747.877742	43.979457
3503.393946	508720.126354	43.984461
3503.516879	508707.813101	43.989466
3503.175540	508696.028549	43.994471
3503.321683	508696.106756	43.999476
3503.218292	508678.264087	44.004481
3503.572000	508660.298560	44.009485
3502.814544	508660.418398	44.014490
3503.112285	508658.448944	44.019495
3503.158261	508636.231665	44.024500
3503.268452	508633.077629	44.029505
3503.461810	508619.640144	44.034509
3503.209243	508619.831961	44.039514
3503.286845	508606.766911	44.044519
3503.604065	508594.625240	44.049524
3503.320207	508580.403074	44.054529
3503.402442	508574.268472	44.059533
3503.386013	508557.828530	44.064538
3503.409732	508536.677090	44.069543
3503.291999	508531.687122	44.074548
3502.598052	508538.626962	44.079553
3502.882498	508526.996352	44.084557
3503.009719	508534.818264	44.089562
3503.083358	508515.075508	44.094567
3503.168952	508496.241513	44.099572
3503.128931	508492.402890	44.104577
3503.126415	508494.831873	44.109581
3502.963389	508491.569214	44.114586
3502.926667	508488.438371	44.119591
3503.024041	508460.951066	44.124596
3503.078546	508457.198682	44.129601
3503.055049	508453.053880	44.134605
3503.212825	508460.870997	44.139610
3503.100484	508451.832704	44.144615
3503.451406	508444.744913	44.149620
3503.273653	508425.750092	44.154625
3503.346506	508420.831155	44.159629
3503.080642	508423.099398	44.164634
3502.807734	508413.529938	44.169639
3503.106556	508408.018757	44.174644
3502.742701	508406.255028	44.179649
3503.189322	508376.233318	44.184653
3502.607482	508373.745139	44.189658
3503.064677	508362.896608	44.194663
3503.082590	508372.101893	44.199668
3502.864165	508374.463830	44.204673
3503.135053	508364.353055	44.209677
3503.195421	508376.131890	44.214682
3503.299844	508343.988695	44.219687
3503.253943	508333.523222	44.224692
3502.779927	508329.044848	44.229697
3502.870587	508324.730192	44.234701
3503.181665	508324.428178	44.239706
3503.217178	508330.746873	44.244711
3502.918194	508307.420040	44.249716
3503.009457	508289.192045	44.254721
3503.222360	508279.748101	44.259725
3503.137083	508284.871657	44.264730
3503.044263	508284.937041	44.269735
3503.155775	508280.416703	44.274740
3502.823879	508268.276210	44.279745
3502.978153	508250.645339	44.284749
3503.355900	508236.520694	44.289754
3502.899744	508234.467973	44.294759
3503.185513	508237.003209	44.299764
3503.010826	508238.093408	44.304769
3503.251393	508232.389004	44.309773
3502.857467	508214.996522	44.314778
3503.121865	508198.866008	44.319783
3503.327000	508204.044875	44.324788
3502.717176	508202.421188	44.329793
3503.332623	508198.782465	44.334797
3503.142130	508199.723383	44.339802
3503.077790	508171.856424	44.344807
3503.074618	508167.354183	44.349812
3502.995530	508169.441156	44.354817
3503.182280	508149.528321	44.359821
3503.078696	508164.318261	44.364826
3502.946521	508143.798104	44.369831
3503.119391	508123.988621	44.374836
3503.005851	508127.548273	44.379841
3502.997998	508122.844384	44.384845
3503.156056	508120.087441	44.389850
3502.958074	508108.279827	44.394855
3502.951500	508116.224265	44.399860
3502.769350	508124.500015	44.404865
3503.173699	508114.772751	44.409869
3503.151727	508097.220174	44.414874
3502.967500	508085.815124	44.419879
3503.133996	508078.199796	44.424884
3502.908523	508080.461699	44.429889
3503.039889	508079.783332	44.434893
3502.984726	508072.253629	44.439898
3503.030712	508059.850886	44.444903
3503.116135	508043.495542	44.449908
3502.721637	508038.700957	44.454913
3503.405241	508035.152616	44.459917
3503.089578	508037.732346	44.464922
3502.935487	508031.078365	44.469927
3502.973479	508029.200488	44.474932
3502.914844	508017.421382	44.479937
3503.058749	508001.866267	44.484941
3502.785908	507996.951253	44.489946
3503.044789	507990.130796	44.494951
3503.105045	507990.981499	44.499956
3502.965361	507998.643463	44.504961
3503.043929	507997.113331	44.509965
3502.911877	507993.845682	44.514970
3503.067034	507983.752975	44.519975
3503.368093	507965.339695	44.524980
3503.068347	507955.217680	44.529985
3503.093689	507957.288173	44.534989
3502.903843	507958.836137	44.539994
3503.125942	507952.578019	44.544999
3503.380500	507924.407284	44.550004
3503.156926	507926.011176	44.555009
3503.275622	507908.385579	44.560013
3503.066213	507905.332518	44.565018
3502.904007	507915.730194	44.570023
3503.328812	507904.178170	44.575028
3503.305324	507876.557250	44.580033
3503.191993	507875.361007	44.585037
3503.101121	507874.060024	44.590042
3503.160409	507871.622222	44.595047
3503.506284	507841.109555	44.600052
3503.208507	507832.757980	44.605057
3503.281723	507819.996595	44.610061
3503.407691	507824.327975	44.615066
3503.297706	507802.842599	44.620071
3503.171699	507785.660313	44.625076
3503.219712	507798.402803	44.630081
3503.275268	507787.667987	44.635085
3503.224801	507774.926118	44.640090
3502.957262	507756.906055	44.645095
3503.342698	507740.958363	44.650100
3502.914807	507749.981465	44.655105
3503.078745	507739.583656	44.660109
3502.910450	507743.354422	44.665114
3502.804475	507736.085579	44.670119
3503.138963	507724.092353	44.675124
3503.272122	507704.845213	44.680129
3503.452408	507698.846588	44.685133
3503.501893	507705.871639	44.690138
3503.287532	507676.712112	44.695143
3503.342506	507657.983231	44.700148
3502.752545	507659.240292	44.705153
3503.069507	507644.315243	44.710157
3503.046978	507657.726728	44.715162
3502.896957	507656.637459	44.720167
3503.041726	507651.504555	44.725172
3502.950733	507628.194523	44.730177
3503.148616	507618.044253	44.735181
3502.732209	507626.154884	44.740186
3502.682913	507622.418723	44.745191
3502.847734	507624.315425	44.750196
3502.818613	507616.326047	44.755201
3503.002977	507616.195837	44.760205
3503.113652	507616.431442	44.765210
3503.101636	507610.109012	44.770215
3503.075352	507591.797667	44.775220
3502.854170	507582.168972	44.780225
3502.936078	507570.822708	44.785229
3502.983089	507580.327392	44.790234
3502.986800	507577.442971	44.795239
3503.348763	507575.817415	44.800244
3502.864791	507582.623256	44.805249
3502.839548	507566.537930	44.810253
3502.916516	507549.677497	44.815258
3503.274229	507535.150679	44.820263
3503.138668	507535.931163	44.825268
3502.933445	507537.633381	44.830273
3503.199267	507522.513927	44.835277
3502.582280	507534.602779	44.840282
3502.897473	507537.892407	44.845287
3502.907594	507524.027668	44.850292
3503.105726	507508.109365	44.855297
3503.117840	507494.396075	44.860301
3502.986785	507491.836515	44.865306
3503.231408	507493.619427	44.870311
3503.172784	507492.920469	44.875316
3503.003926	507485.813248	44.880321
3503.038134	507459.548632	44.885325
3502.972009	507454.044233	44.890330
3502.823471	507448.805839	44.895335
3503.272874	507449.443275	44.900340
3503.117333	507456.399640	44.905345
3503.284226	507445.647015	44.910349
3502.869752	507429.268907	44.915354
3502.988203	507410.428532	44.920359
3503.089188	507408.540632	44.925364
3502.626624	507406.691207	44.930369
3503.117576	507400.491589	44.935373
3502.938437	507401.987313	44.940378
3502.698020	507402.480798	44.945383
3503.258675	507403.859595	44.950388
3503.033608	507408.044177	44.955393
3503.283704	507389.486550	44.960397
3503.309630	507375.770982	44.965402
3502.955099	507367.175169	44.970407
3503.190317	507362.280865	44.975412
3503.208972	507369.412118	44.980417
3503.190460	507343.762815	44.985421
3502.748825	507333.662860	44.990426
3502.667993	507328.565517	44.995431
3502.950570	507321.032701	45.000436
3502.894335	507322.104235	45.005441
3503.035160	507316.921259	45.010445
3502.964152	507329.278136	45.015450
3502.784127	507326.726291	45.020455
3503.042743	507316.819228	45.025460
3503.050085	507312.871663	45.030465
3503.242307	507286.885389	45.035469
3503.214800	507287.547612	45.040474
3502.956902	507277.115005	45.045479
3503.002029	507277.107992	45.050484
3502.979536	507277.465844	45.055489
3502.995748	507281.005162	45.060493
3503.172477	507265.494792	45.065498
3502.886217	507254.914864	45.070503
3502.777990	507242.181729	45.075508
3502.887944	507247.628912	45.080513
3503.347179	507240.978881	45.085517
3503.350653	507246.695877	45.090522
3503.057619	507234.649703	45.095527
3503.398541	507211.321439	45.100532
3503.282877	507206.684936	45.105537
3503.067166	507199.230824	45.110541
3503.102638	507206.561874	45.115546
3502.756011	507184.404774	45.120551
3503.137780	507168.305344	45.125556
3503.187837	507162.731893	45.130561
3503.018487	507161.443259	45.135565
3503.002017	507154.261218	45.140570
3502.736410	507159.312415	45.145575
3502.852548	507157.928063	45.150580
3503.004965	507161.496475	45.155585
3503.078981	507146.255216	45.160589
3503.200369	507135.964964	45.165594
3502.910831	507132.570250	45.170599
3503.421653	507123.533961	45.175604
3502.890776	507124.680526	45.180609
3502.957905	507120.824661	45.185613
3503.262951	507113.490593	45.190618
3503.223747	507103.023314	45.195623
3503.133300	507089.983675	45.200628
3503.182560	507088.154513	45.205633
3503.406195	507079.568369	45.210637
3503.547044	507063.253934	45.215642
3503.013390	507050.537301	45.220647
3503.269817	507033.799793	45.225652
3502.878651	507042.665665	45.230657
3503.113119	507039.542293	45.235661
3503.381208	507018.451561	45.240666
3502.874731	507003.554911	45.245671
3502.876869	507000.518851	45.250676
3503.036426	506998.975831	45.255681
3503.390857	506989.104034	45.260685
3502.858403	506992.325350	45.265690
3503.102493	506981.914418	45.270695
3503.364251	506959.003105	45.275700
3503.043694	506962.342729	45.280705
3503.123983	506958.838931	45.285709
3503.170531	506957.313769	45.290714
3503.049707	506955.106695	45.295719
3503.059383	506930.818456	45.300724
3502.840926	506917.697724	45.305729
3503.133152	506908.544080	45.310733
3502.663973	506920.205216	45.315738
3502.766376	506915.534169	45.320743
3503.308852	506919.091579	45.325748
3502.881284	506920.019438	45.330753
3503.122322	506906.623682	45.335757
3502.987882	506887.316731	45.340762
3502.905597	506874.275639	45.345767
3502.866182	506872.055687	45.350772
3502.893434	506870.280578	45.355777
3503.185705	506857.888643	45.360781
3502.802258	506867.107569	45.365786
3503.083790	506875.108238	45.370791
3503.219222	506863.196476	45.375796
3503.012094	506847.493412	45.380801
3503.141207	506831.838385	45.385805
3503.169412	506843.522156	45.390810
3502.852291	506834.363586	45.395815
3503.137433	506828.651676	45.400820
3503.089918	506823.801907	45.405825
3503.278045	506811.628791	45.410829
3503.047735	506798.712233	45.415834
3503.056495	506796.737648	45.420839
3503.344028	506789.305015	45.425844
3503.283416	506790.984449	45.430849
3503.013499	506761.983951	45.435853
3503.273299	506749.647669	45.440858
3502.877804	506747.635775	45.445863
3503.237857	506741.608407	45.450868
3502.865548	506738.074903	45.455873
3503.347038	506735.114827	45.460877
3503.352459	506719.175659	45.465882
3502.908829	506711.150180	45.470887
3503.011021	506700.457917	45.475892
3502.722747	506700.857788	45.480897
3502.775486	506702.316922	45.485901
3502.912196	506709.075601	45.490906
3502.761878	506709.706659	45.495911
3502.914313	506704.369870	45.500916
3502.799763	506704.388095	45.505921
3503.085709	506689.214135	45.510925
3503.116506	506684.604941	45.515930
3503.129015	506661.732630	45.520935
3503.349731	506659.471537	45.525940
3502.934289	506658.828941	45.530945
3503.183337	506664.051931	45.535949
3503.149208	506639.871404	45.540954
3502.877225	506630.806789	45.545959
3503.103339	506623.535588	45.550964
3502.997839	506628.865224	45.555969
3503.020490	506623.599522	45.560973
3502.985750	506623.807527	45.565978
3502.828367	506629.752545	45.570983
3503.117981	506615.994698	45.575988
3502.889990	506588.151048	45.580993
3503.064324	506577.852095	45.585997
3502.870534	506578.085239	45.591002
3502.757046	506572.689242	45.596007
3502.795564	506569.697955	45.601012
3502.778323	506571.927141	45.606017
3503.058276	506572.490197	45.611021
3503.216681	506572.060492	45.616026
3503.034558	506576.491479	45.621031
3503.290923	506557.628378	45.626036
3502.842156	506556.434460	45.631041
3502.979033	506542.650097	45.636045
3502.871713	506546.613880	45.641050
3503.233119	506537.904496	45.646055
3503.234755	506535.627414	45.651060
3502.974616	506521.298599	45.656065
3503.354015	506500.543835	45.661069
3503.268666	506497.217920	45.666074
3502.948640	506492.461729	45.671079
3503.230440	506490.545151	45.676084
3503.314387	506482.132587	45.681089
3503.358519	506452.879538	45.686093
3503.245520	506464.181090	45.691098
3503.129153	506464.098405	45.696103
3503.417018	506450.138307	45.701108
3503.332035	506435.478143	45.706113
3503.179571	506415.262731	45.711117
3503.513358	506419.865212	45.716122
3502.960315	506404.823608	45.721127
3503.438553	506380.156945	45.726132
3502.916188	506374.117121	45.731137
3503.167199	506372.559592	45.736141
3503.219596	506369.464877	45.741146
3503.219352	506358.940392	45.746151
3502.951627	506333.278380	45.751156
3502.869604	506331.571086	45.756161
3503.367768	506328.709506	45.761165
3503.199695	506324.536444	45.766170
3503.087674	506325.161461	45.771175
3503.168827	506313.055502	45.776180
3502.982267	506296.943892	45.781185
3503.257388	506290.879194	45.786189
3503.110804	506282.047573	45.791194
3503.155621	506286.948760	45.796199
3503.394971	506284.988270	45.801204
3503.031834	506264.704781	45.806209
3503.005464	506239.864676	45.811213
3503.178529	506241.001234	45.816218
3503.098271	506243.594619	45.821223
3503.221543	506244.081252	45.826228
3503.077077	506230.138710	45.831233
3503.006648	506203.888726	45.836237
3502.917716	506210.430265	45.841242
3502.913173	506201.980952	45.846247
3503.233998	506190.393623	45.851252
3502.901284	506201.375875	45.856257
3502.990436	506192.051552	45.861261
3503.166753	506195.869386	45.866266
3503.186371	506169.200320	45.871271
3503.663803	506152.730631	45.876276
3503.291500	506152.991994	45.881281
3502.946168	506138.069128	45.886285
3502.831653	506128.523962	45.891290
3503.287565	506128.806223	45.896295
3503.368536	506108.098158	45.901300
3503.143302	506101.758277	45.906305
3503.135131	506101.658488	45.911309
3503.297843	506094.700687	45.916314
3503.275313	506067.532127	45.921319
3503.293183	506066.972821	45.926324
3503.130881	506064.519188	45.931329
3503.111150	506049.595383	45.936333
3503.149775	506040.734367	45.941338
3502.973163	506021.281315	45.946343
3503.433128	506012.252489	45.951348
3502.950800	506019.109279	45.956353
3503.217344	506015.575853	45.961357
3503.157013	506000.658423	45.966362
3502.947461	505980.704529	45.971367
3502.885551	505977.374809	45.976372
3502.628079	505975.492809	45.981377
3503.112571	505961.956646	45.986381
3502.906186	505973.981683	45.991386
3502.922599	505967.704760	45.996391
3503.016279	505962.933635	46.001396
3502.959050	505970.583462	46.006401
3503.014215	505956.001942	46.011405
3503.105336	505937.670291	46.016410
3502.899994	505937.652265	46.021415
3503.078838	505936.055503	46.026420
3502.917221	505937.953386	46.031425
3503.275339	505931.369440	46.036429
3502.672360	505933.337082	46.041434
3502.753217	505939.750686	46.046439
3503.078133	505921.331464	46.051444
3503.200468	505896.922770	46.056449
3503.022042	505894.168057	46.061453
3503.093706	505889.147388	46.066458
3502.719395	505883.893602	46.071463
3503.098596	505891.019080	46.076468
3502.867860	505898.089155	46.081473
3503.127800	505884.588423	46.086477
3502.896204	505868.230529	46.091482
3502.934408	505862.860936	46.096487
3503.424108	505844.921597	46.101492
3503.368380	505853.785657	46.106497
3503.099923	505850.792163	46.111501
3503.117653	505831.105779	46.116506
3502.833453	505819.310225	46.121511
3502.949453	505806.085187	46.126516
3502.815354	505804.335471	46.131521
3503.091801	505800.699235	46.136525
3502.983822	505815.491877	46.141530
3502.851680	505807.922753	46.146535
3502.970497	505807.549888	46.151540
3503.187532	505802.303814	46.156545
3502.574277	505780.844869	46.161549
3502.870448	505783.783634	46.166554
3502.940366	505776.334363	46.171559
3502.948885	505769.653808	46.176564
3502.599728	505778.918491	46.181569
3502.983515	505769.901581	46.186573
3503.001794	505773.795087	46.191578
3503.073270	505776.668166	46.196583
3503.017651	505780.927557	46.201588
3503.183608	505766.834377	46.206593
3502.993171	505749.306043	46.211597
3502.810579	505742.402678	46.216602
3502.966293	505735.901250	46.221607
3503.111275	505728.541297	46.226612
3502.806812	505738.254347	46.231617
3502.835678	505735.618648	46.236621
3502.984212	505739.997586	46.241626
3503.132820	505733.800887	46.246631
3503.150653	505715.227579	46.251636
3502.927882	505700.082559	46.256641
3503.002786	505690.153005	46.261645
3502.937372	505683.888912	46.266650
3502.827157	505687.802747	46.271655
3503.004583	505674.719704	46.276660
3502.968474	505697.293679	46.281665
3503.229719	505678.327652	46.286669
3503.248362	505654.086809	46.291674
3502.836684	505644.891952	46.296679
3503.096952	505642.624477	46.301684
3502.983999	505636.418482	46.306689
3503.099598	505628.557117	46.311693
3503.217095	505645.085315	46.316698
3502.970909	505623.568159	46.321703
3503.161019	505606.485548	46.326708
3503.027615	505604.634499	46.331713
3502.989494	505595.380574	46.336717
3503.108580	505600.624426	46.341722
3503.021546	505595.729959	46.346727
3503.207853	505571.411900	46.351732
3502.917108	505560.022017	46.356737
3503.155464	505555.126710	46.361741
3502.989819	505565.981752	46.366746
3503.242824	505561.084132	46.371751
3503.056294	505551.904242	46.376756
3502.948215	505541.801118	46.381761
3502.855332	505522.941494	46.386765
3502.822466	505512.067439	46.391770
3502.692547	505517.300071	46.396775
3503.075189	505519.213181	46.401780
3503.077292	505525.740589	46.406785
3502.880915	505514.993583	46.411789
3502.981594	505511.030855	46.416794
3502.952043	505520.498169	46.421799
3503.026418	505515.173353	46.426804
3502.853200	505497.237230	46.431809
3503.087358	505479.995727	46.436813
3503.003771	505473.683829	46.441818
3503.150589	505473.053523	46.446823
3503.083091	505471.849867	46.451828
3502.596011	505474.811277	46.456833
3502.762814	505476.556098	46.461837
3502.963768	505486.796627	46.466842
3502.861600	505482.005723	46.471847
3503.160782	505453.115494	46.476852
3502.666227	505446.160114	46.481857
3502.867603	505427.861101	46.486861
3503.257187	505426.230985	46.491866
3502.929950	505433.670714	46.496871
3503.034224	505436.943481	46.501876
3503.110144	505439.107486	46.506881
3503.117289	505427.215015	46.511885
3502.958833	505401.180140	46.516890
3502.865313	505386.773450	46.521895
3502.963389	505388.023121	46.526900
3502.696500	505395.655737	46.531905
3502.702433	505394.794684	46.536909
3503.003476	505387.814738	46.541914
3502.717374	505389.681753	46.546919
3502.977131	505387.869744	46.551924
3502.733006	505397.472243	46.556929
3503.212723	505387.680943	46.561933
3502.796213	505396.905871	46.566938
3503.149598	505378.785189	46.571943
3503.290162	505357.510189	46.576948
3503.222050	505354.383739	46.581953
3503.213677	505348.565929	46.586957
3503.114732	505344.280500	46.591962
3503.027564	505333.566723	46.596967
3503.153246	505303.134998	46.601972
3502.946250	505300.232899	46.606977
3503.268261	505292.237554	46.611981
3502.743510	505298.696510	46.616986
3502.822570	505302.125095	46.621991
3503.157022	505305.715722	46.626996
3502.769601	505299.401180	46.632001
3502.723092	505274.006252	46.637005
3503.037478	505272.489212	46.642010
3503.051073	505262.872719	46.647015
3503.184869	505259.461328	46.652020
3502.925338	505262.285603	46.657025
3502.938405	505257.274014	46.662029
3503.022814	505259.892122	46.667034
3502.689908	505260.703896	46.672039
3503.319515	505250.180394	46.677044
3503.063738	505234.635365	46.682049
3503.092491	505213.782682	46.687053
3502.975484	505215.622989	46.692058
3502.714576	505210.705292	46.697063
3503.250596	505215.478542	46.702068
3503.015910	505223.460361	46.707073
3503.012947	505203.422319	46.712077
3502.896803	505190.638326	46.717082
3502.926547	505186.990353	46.722087
3503.012478	505173.668382	46.727092
3503.161717	505174.758174	46.732097
3503.098252	505167.127314	46.737101
3502.896928	505176.874977	46.742106
3502.992872	505169.623744	46.747111
3502.995312	505151.861912	46.752116
3502.894546	505134.166976	46.757121
3502.966307	505132.485861	46.762125
3503.088352	505130.391975	46.767130
3503.012822	505131.213679	46.772135
3502.920589	505131.025965	46.777140
3502.842377	505140.349368	46.782145
3502.575157	505140.239914	46.787149
3502.781395	505141.523111	46.792154
3502.795759	505136.764296	46.797159
3503.231871	505131.533999	46.802164
3502.783587	505121.686813	46.807169
3502.917673	505100.716140	46.812173
3503.069136	505105.094776	46.817178
3503.028269	505100.951915	46.822183
3502.943818	505114.020934	46.827188
3503.039966	505118.509515	46.832193
3502.826511	505107.005912	46.837197
3502.930332	505104.307669	46.842202
3503.003645	505079.348945	46.847207
3503.204214	505058.468920	46.852212
3502.712793	505068.009479	46.857217
3502.946940	505059.977312	46.862221
3502.874310	505063.379315	46.867226
3502.925629	505066.356904	46.872231
3502.917065	505061.146265	46.877236
3502.873446	505063.076195	46.882241
3503.072935	505053.025381	46.887245
3503.211765	505026.133309	46.892250
3502.713521	505014.624054	46.897255
3503.183420	505000.684629	46.902260
3502.761772	505015.476923	46.907265
3502.900064	505013.178042	46.912269
3503.197002	505004.174465	46.917274
3503.176446	505006.353772	46.922279
3503.463539	504992.291423	46.927284
3503.139986	504978.932818	46.932289
3503.136801	504966.839253	46.937293
3503.246107	504965.658220	46.942298
3503.014021	504965.897436	46.947303
3503.202155	504948.004840	46.952308
3502.911133	504935.450713	46.957313
3502.994397	504923.950696	46.962317
3503.189989	504921.389730	46.967322
3503.164146	504931.261604	46.972327
3502.963840	504923.298041	46.977332
3502.953942	504921.376795	46.982337
3503.430265	504899.289117	46.987341
3503.245884	504888.438620	46.992346
3503.206008	504885.965469	46.997351
3503.286184	504875.022547	47.002356
3502.950242	504861.412791	47.007361
3503.350981	504842.879241	47.012365
3503.115561	504836.439298	47.017370
3503.190166	504839.008415	47.022375
3503.098129	504829.965020	47.027380
3503.157323	504821.960396	47.032385
3503.076631	504798.897950	47.037389
3503.296999	504800.330751	47.042394
3503.159703	504798.986268	47.047399
3503.013834	504801.438426	47.052404
3503.068531	504792.321216	47.057409
3503.227934	504762.794088	47.062413
3503.370385	504759.583647	47.067418
3503.433108	504754.159233	47.072423
3503.356074	504746.479730	47.077428
3503.236046	504728.483803	47.082433
3503.295558	504709.852232	47.087437
3503.168565	504701.775773	47.092442
3503.078572	504704.219113	47.097447
3503.323556	504688.645053	47.102452
3502.884805	504676.721338	47.107457
3503.020694	504663.795916	47.112461
3503.478933	504660.231920	47.117466
3503.296207	504658.287356	47.122471
3503.217218	504648.179116	47.127476
3502.794520	504629.370653	47.132481
3503.031567	504617.896733	47.137485
3502.817346	504613.578739	47.142490
3503.072308	504618.396577	47.147495
3503.044001	504610.759917	47.152500
3502.949782	504614.216024	47.157505
3503.016410	504606.361939	47.162509
3503.095778	504597.594958	47.167514
3502.899844	504580.471151	47.172519
3503.361815	504576.957153	47.177524
3503.019567	504571.950921	47.182529
3503.310809	504566.186705	47.187533
3503.128813	504570.112135	47.192538
3502.973604	504553.740931	47.197543
3502.967407	504531.627844	47.202548
3502.665504	504534.610747	47.207553
3502.855435	504525.725046	47.212557
3503.133047	504519.052085	47.217562
3502.776762	504514.705915	47.222567
3502.799343	504517.789349	47.227572
3502.442729	504521.236342	47.232577
3503.025428	504519.322599	47.237581
3503.209140	504516.054987	47.242586
3502.851774	504516.516427	47.247591
3503.185717	504495.513441	47.252596
3502.862846	504483.976116	47.257601
3502.743724	504487.436184	47.262605
3502.995858	504477.832162	47.267610
3503.177228	504475.577007	47.272615
3503.420609	504477.967688	47.277620
3503.208237	504483.213661	47.282625
3503.387475	504446.142759	47.287629
3503.136564	504437.174875	47.292634
3502.954493	504436.141071	47.297639
3503.056846	504436.934691	47.302644
3502.968752	504438.719905	47.307649
3502.828620	504416.627841	47.312653
3503.107872	504410.005185	47.317658
3503.188433	504414.648226	47.322663
3503.045056	504399.691945	47.327668
3502.829425	504403.217889	47.332673
3503.003300	504399.951810	47.337677
3503.281518	504394.898066	47.342682
3503.108187	504379.035612	47.347687
3502.802353	504363.244693	47.352692
3503.008765	504358.556522	47.357697
3503.482158	504352.004370	47.362701
3503.208932	504354.021273	47.367706
3503.313452	504344.238088	47.372711
3503.201582	504323.710199	47.377716
3502.626211	504317.779241	47.382721
3502.755645	504314.317750	47.387725
3503.141301	504313.244812	47.392730
3502.752964	504313.711152	47.397735
3502.646364	504311.197860	47.402740
3502.765066	504312.899796	47.407745
3503.009759	504308.863430	47.412749
3503.015014	504313.467794	47.417754
3503.066592	504306.223216	47.422759
3502.829398	504273.620422	47.427764
3502.859914	504276.095380	47.432769
3502.936313	504269.605943	47.437773
3502.925926	504260.498742	47.442778
3502.918885	504270.418623	47.447783
3502.658185	504268.992393	47.452788
3502.750912	504275.809577	47.457793
3502.791356	504273.070618	47.462797
3502.911062	504274.519373	47.467802
3502.829576	504262.488301	47.472807
3502.941809	504264.798529	47.477812
3502.703742	504277.588820	47.482817
3502.994669	504269.446106	47.487821
3503.078673	504239.069721	47.492826
3503.117914	504227.373782	47.497831
3503.433558	504222.364678	47.502836
3502.990780	504236.199465	47.507841
3503.117493	504221.959425	47.512845
3503.097916	504213.460918	47.517850
3502.863576	504196.190987	47.522855
3502.891736	504186.065544	47.527860
3502.870594	504188.498073	47.532865
3503.026546	504173.393078	47.537869
3503.092684	504178.645728	47.542874
3502.606866	504188.894356	47.547879
3502.710864	504176.732699	47.552884
3502.594784	504187.631367	47.557889
3502.822685	504184.306105	47.562893
3502.961401	504179.780403	47.567898
3502.844800	504189.565830	47.572903
3502.938285	504162.578386	47.577908
3502.979932	504153.260482	47.582913
3503.054505	504135.587428	47.587917
3503.070666	504133.813793	47.592922
3503.121235	504144.584938	47.597927
3503.111035	504137.097025	47.602932
3502.973533	504137.017667	47.607937
3503.107553	504122.169123	47.612941
3502.890058	504101.252821	47.617946
3502.535983	504100.853451	47.622951
3503.186888	504093.564665	47.627956
3502.701408	504090.301531	47.632961
3502.628750	504091.527676	47.637965
3502.902762	504090.624188	47.642970
3502.578645	504088.904332	47.647975
3503.004131	504088.989020	47.652980
3502.841985	504094.227170	47.657985
3503.062075	504084.982239	47.662989
3502.967647	504093.195433	47.667994
3502.940515	504092.339542	47.672999
3503.279272	504061.821373	47.678004
3502.887907	504058.948205	47.683009
3502.863244	504057.838893	47.688013
3503.523796	504052.420985	47.693018
3503.009133	504053.109722	47.698023
3503.126167	504043.071361	47.703028
3503.054779	504022.081265	47.708033
3503.275589	504017.137698	47.713037
3502.971192	504009.949261	47.718042
3502.441058	504008.717412	47.723047
3503.116806	504006.586484	47.728052
3503.078114	504000.418775	47.733057
3503.032030	504005.132547	47.738061
3502.819603	503985.733489	47.743066
3503.007726	503972.293239	47.748071
3502.731171	503970.161003	47.753076
3502.846837	503968.219806	47.758081
3503.110062	503952.591604	47.763085
3503.140736	503960.532056	47.768090
3502.551116	503968.266907	47.773095
3502.927505	503956.821138	47.778100
3502.828416	503966.705133	47.783105
3503.020747	503967.180917	47.788109
3502.913693	503963.453098	47.793114
3502.881868	503948.782438	47.798119
3503.420862	503931.288805	47.803124
3502.934988	503932.428452	47.808129
3503.232923	503930.154805	47.813133
3503.289133	503925.085408	47.818138
3503.088751	503910.896815	47.823143
3503.309371	503892.289517	47.828148
3502.990907	503882.319896	47.833153
3503.204620	503879.249851	47.838157
3503.147438	503884.926932	47.843162
3503.190337	503873.078359	47.848167
3503.209639	503846.253973	47.853172
3502.863017	503847.877681	47.858177
3502.823217	503845.606797	47.863181
3502.995769	503836.419855	47.868186
3502.592537	503839.165857	47.873191
3503.142140	503835.081190	47.878196
3502.801178	503832.250624	47.883201
3503.109539	503827.495593	47.888205
3502.894512	503805.060348	47.893210
3502.746865	503794.355186	47.898215
3503.129811	503779.315188	47.903220
3502.754098	503790.457566	47.908225
3503.080448	503785.396039	47.913229
3503.104672	503785.038084	47.918234
3502.742779	503790.459716	47.923239
3503.097816	503790.757968	47.928244
3503.124573	503793.537229	47.933249
3503.338163	503759.900702	47.938253
3503.118732	503758.720941	47.943258
3502.645530	503757.783716	47.948263
3503.037238	503746.588423	47.953268
3502.827640	503753.656021	47.958273
3503.082079	503740.559360	47.963277
3502.957482	503744.071047	47.968282
3502.757196	503747.493482	47.973287
3502.880260	503728.952037	47.978292
3503.085617	503719.203173	47.983297
3503.131050	503711.756892	47.988301
3503.230897	503705.567183	47.993306
3503.188608	503706.434306	47.998311
3503.493075	503700.920751	48.003316
3503.313833	503683.236750	48.008321
3503.108597	503674.817932	48.013325
3503.036976	503664.960994	48.018330
3502.934507	503665.382167	48.023335
3503.239606	503662.398854	48.028340
3502.838363	503647.229652	48.033345
3502.872197	503625.969416	48.038349
3502.847864	503621.823591	48.043354
3502.499343	503618.083256	48.048359
3502.765670	503616.776102	48.053364
3502.999949	503624.077239	48.058369
3503.043073	503622.349898	48.063373
3503.174561	503621.165271	48.068378
3503.111661	503620.922297	48.073383
3503.141815	503606.190947	48.078388
3502.761820	503598.457608	48.083393
3502.874911	503577.589645	48.088397
3502.908201	503577.129038	48.093402
3502.786604	503577.047162	48.098407
3503.145413	503575.118100	48.103412
3503.257427	503577.124810	48.108417
3503.067526	503568.298658	48.113421
3503.171665	503571.774227	48.118426
3502.851516	503554.213581	48.123431
3502.819306	503550.271414	48.128436
3503.052131	503548.362261	48.133441
3503.276109	503540.837082	48.138445
3502.958686	503537.850925	48.143450
3503.167500	503539.032620	48.148455
3503.140886	503516.466012	48.153460
3503.437513	503496.834132	48.158465
3503.225813	503492.819106	48.163469
3503.307068	503486.581651	48.168474
3503.076368	503488.844968	48.173479
3503.352700	503451.452972	48.178484
3503.030935	503455.046487	48.183489
3503.178896	503442.219472	48.188493
3502.962066	503444.075741	48.193498
3503.045688	503453.273247	48.198503
3503.192419	503424.555591	48.203508
3502.742253	503407.420210	48.208513
3502.829736	503395.867916	48.213517
3502.645512	503392.708858	48.218522
3502.567253	503399.249761	48.223527
3503.317550	503390.376134	48.228532
3503.124244	503398.757104	48.233537
3503.245877	503395.701529	48.238541
3503.114304	503392.028071	48.243546
3502.971799	503377.020171	48.248551
3503.101232	503362.779005	48.253556
3502.854560	503359.123732	48.258561
3502.757503	503351.345564	48.263565
3503.030512	503356.717588	48.268570
3502.840446	503349.409592	48.273575
3503.312043	503351.916182	48.278580
3503.151402	503356.142154	48.283585
3503.086457	503327.609620	48.288589
3502.836694	503306.444429	48.293594
3502.860695	503308.009607	48.298599
3503.126284	503300.528356	48.303604
3502.799372	503304.628796	48.308609
3502.710323	503305.958802	48.313613
3502.847937	503298.345953	48.318618
3502.825436	503309.179768	48.323623
3502.934403	503295.194822	48.328628
3502.923431	503307.899317	48.333633
3502.998069	503267.299889	48.338637
3503.091533	503269.511998	48.343642
3502.810346	503269.961427	48.348647
3503.011041	503255.860736	48.353652
3502.905955	503263.418095	48.358657
3502.940805	503265.032171	48.363661
3503.062104	503262.482707	48.368666
3503.015728	503261.933467	48.373671
3503.098414	503234.187179	48.378676
3503.202873	503228.300223	48.383681
3503.049023	503211.775725	48.388685
3503.385915	503220.224805	48.393690
3502.746450	503219.465653	48.398695
3502.901891	503215.594969	48.403700
3502.940413	503215.133525	48.408705
3502.809407	503187.775198	48.413709
3503.025371	503179.390787	48.418714
3503.051796	503183.941493	48.423719
3503.057912	503171.389742	48.428724
3502.915031	503173.436786	48.433729
3502.747475	503182.117440	48.438733
3502.898446	503178.045020	48.443738
3502.998186	503183.748134	48.448743
3503.235964	503174.651755	48.453748
3503.039669	503155.856530	48.458753
3502.839824	503146.879913	48.463757
3502.873961	503141.965605	48.468762
3502.897014	503131.334275	48.473767
3503.071540	503132.470809	48.478772
3502.790206	503135.045826	48.483777
3503.354080	503135.968996	48.488781
3503.233758	503110.177726	48.493786
3502.862789	503103.353697	48.498791
3503.016362	503092.802932	48.503796
3502.934308	503097.168372	48.508801
3502.987203	503086.026210	48.513805
3503.018817	503090.323077	48.518810
3502.749446	503088.088379	48.523815
3502.951482	503091.295526	48.528820
3502.643067	503093.368742	48.533825
3502.749787	503071.691446	48.538829
3502.818859	503057.915052	48.543834
3502.585671	503047.779651	48.548839
3503.179489	503044.548167	48.553844
3502.926680	503045.752248	48.558849
3502.744231	503042.441020	48.563853
3502.669112	503055.004010	48.568858
3502.703609	503044.472036	48.573863
3502.770587	503041.475646	48.578868
3502.562786	503045.506712	48.583873
3502.860713	503039.437287	48.588877
3503.159083	503033.013528	48.593882
3502.768593	503046.891592	48.598887
3502.960505	503042.610235	48.603892
3502.826355	503049.818017	48.608897
3503.016071	503043.158391	48.613901
3502.768925	503030.393524	48.618906
3502.792771	503018.243733	48.623911
3503.161326	503002.496822	48.628916
3502.644396	503018.672296	48.633921
3502.879469	503008.918343	48.638925
3502.961357	503006.476289	48.643930
3502.939003	503015.184685	48.648935
3502.975025	503000.755554	48.653940
3503.046821	503000.288846	48.658945
3503.111108	502999.469062	48.663949
3503.212813	502976.830870	48.668954
3502.922597	502969.083063	48.673959
3503.256787	502962.603008	48.678964
3502.823469	502964.645371	48.683969
3502.897850	502963.115462	48.688973
3502.983621	502959.863043	48.693978
3502.941664	502958.958831	48.698983
3502.909837	502936.999612	48.703988
3502.844688	502927.799156	48.708993
3503.112309	502919.457067	48.713997
3503.097779	502926.139900	48.719002
3502.994985	502927.370889	48.724007
3502.936595	502920.294947	48.729012
3503.028636	502927.517638	48.734017
3502.838372	502921.778380	48.739021
3502.736751	502906.966054	48.744026
3502.827489	502905.382945	48.749031
3502.854499	502882.098518	48.754036
3503.011340	502879.593991	48.759041
3503.147607	502872.436655	48.764045
3502.951383	502866.850149	48.769050
3502.703841	502874.025315	48.774055
3503.240156	502868.829123	48.779060
3502.916993	502877.079037	48.784065
3502.831877	502866.110378	48.789069
3503.053356	502845.882338	48.794074
3502.891874	502841.555568	48.799079
3502.921987	502827.835762	48.804084
3502.757338	502832.113103	48.809089
3503.064823	502835.657897	48.814093
3503.033155	502835.966679	48.819098
3502.837213	502838.831899	48.824103
3502.972339	502824.842445	48.829108
3502.901720	502829.003706	48.834113
3502.910900	502822.271312	48.839117
3502.937382	502798.835029	48.844122
3502.750654	502794.714677	48.849127
3503.158775	502787.817997	48.854132
3502.845077	502789.335376	48.859137
3502.773452	502781.704766	48.864141
3502.830582	502786.655599	48.869146
3502.830305	502797.739264	48.874151
3502.964226	502789.063978	48.879156
3503.072376	502782.973851	48.884161
3502.926301	502775.911711	48.889165
3502.967677	502764.467509	48.894170
3502.838798	502753.859964	48.899175
3503.033773	502743.353056	48.904180
3502.651762	502751.359281	48.909185
3502.749472	502743.651281	48.914189
3502.915539	502747.775151	48.919194
3502.722403	502746.388725	48.924199
3502.943422	502742.710012	48.929204
3502.918165	502741.550100	48.934209
3502.611027	502740.738399	48.939213
3502.838448	502736.552575	48.944218
3502.557854	502746.567163	48.949223
3502.771838	502740.865172	48.954228
3502.659504	502748.626336	48.959233
3502.667113	502738.250258	48.964237
3503.063984	502737.934603	48.969242
3502.576578	502747.425171	48.974247
3502.912112	502739.224091	48.979252
3502.760239	502723.508578	48.984257
3502.562481	502715.492996	48.989261
3502.617425	502708.854545	48.994266
3502.731782	502705.091463	48.999271
3503.036980	502697.198817	49.004276
3502.733312	502699.372548	49.009281
3502.714143	502700.084236	49.014285
3502.681659	502713.045610	49.019290
3502.754049	502701.849514	49.024295
3503.016315	502695.279510	49.029300
3502.768173	502698.608492	49.034305
3502.763716	502696.686142	49.039309
3502.901453	502693.324240	49.044314
3502.719689	502694.365287	49.049319
3503.242653	502695.446778	49.054324
3502.914134	502699.446391	49.059329
3503.083216	502693.295993	49.064333
3502.829073	502674.964887	49.069338
3502.703781	502672.555533	49.074343
3503.055482	502666.173822	49.079348
3502.929785	502666.598689	49.084353
3502.707525	502653.222295	49.089357
3502.747893	502661.060583	49.094362
3502.670605	502656.619240	49.099367
3502.891382	502659.013745	49.104372
3502.988062	502662.693113	49.109377
3503.018483	502658.335967	49.114381
3503.352172	502652.615028	49.119386
3502.966038	502636.430363	49.124391
3503.113823	502623.552170	49.129396
3502.847710	502617.015039	49.134401
3502.752217	502618.599165	49.139405
3503.132421	502612.465981	49.144410
3503.140391	502613.274603	49.149415
3503.274982	502604.852171	49.154420
3503.170642	502591.305262	49.159425
3502.897064	502575.153360	49.164429
3503.034660	502566.932876	49.169434
3502.645640	502572.561608	49.174439
3503.044000	502571.891443	49.179444
3503.008700	502571.998363	49.184449
3502.926735	502574.643170	49.189453
3502.788887	502576.993148	49.194458
3502.469107	502580.434694	49.199463
3503.169331	502563.723987	49.204468
3503.006244	502549.781450	49.209473
3502.951776	502518.057499	49.214477
3503.139050	502524.607368	49.219482
3502.998018	502525.439545	49.224487
3503.172272	502518.427892	49.229492
3503.099376	502528.257945	49.234497
3503.165378	502521.668287	49.239501
3503.028602	502497.346420	49.244506
3502.787109	502502.648194	49.249511
3503.219611	502488.611473	49.254516
3502.922264	502491.037282	49.259521
3502.799686	502500.369098	49.264525
3502.894708	502481.830772	49.269530
3502.612000	502488.707990	49.274535
3502.961350	502478.277745	49.279540
3503.018422	502477.610909	49.284545
3502.816458	502450.920588	49.289549
3502.867805	502440.537422	49.294554
3502.513279	502438.923426	49.299559
3502.673464	502433.887778	49.304564
3502.746094	502426.132992	49.309569
3502.611607	502431.316653	49.314573
3502.855566	502430.923940	49.319578
3502.891055	502434.106921	49.324583
3502.788362	502435.186095	49.329588
3502.580080	502437.091728	49.334593
3502.568972	502431.931321	49.339597
3502.870358	502433.300903	49.344602
3502.768554	502434.936654	49.349607
3502.721721	502436.664938	49.354612
3502.881189	502439.372826	49.359617
3502.794598	502437.615261	49.364621
3502.961779	502436.880409	49.369626
3502.707133	502434.845742	49.374631
3503.113419	502433.263329	49.379636
3503.060418	502441.167082	49.384641
3502.812105	502403.855785	49.389645
3503.273823	502396.596207	49.394650
3502.537501	502400.559121	49.399655
3502.770012	502396.271192	49.404660
3502.745929	502397.135501	49.409665
3502.898940	502397.263269	49.414669
3502.971264	502396.948294	49.419674
3502.610520	502402.218336	49.424679
3502.787171	502397.281296	49.429684
3502.497270	502402.691972	49.434689
3502.324346	502398.265681	49.439693
3502.663216	502399.275066	49.444698
3502.286757	502407.432401	49.449703
3502.651371	502394.165495	49.454708
3502.806597	502403.301623	49.459713
3502.882167	502397.115291	49.464717
3503.228558	502400.046695	49.469722
3503.079374	502401.183831	49.474727
3503.143391	502399.503679	49.479732
3502.907778	502379.094296	49.484737
3502.686884	502361.111883	49.489741
3502.807057	502351.072062	49.494746
3502.745857	502356.497216	49.499751
3503.004075	502352.255824	49.504756
3502.694173	502355.948906	49.509761
3502.593833	502351.561742	49.514765
3502.572086	502352.375073	49.519770
3502.447976	502355.785736	49.524775
3502.620125	502351.962834	49.529780
3502.529803	502346.663089	49.534785
3502.590657	502351.360402	49.539789
3502.877933	502343.672876	49.544794
3502.776175	502354.114918	49.549799
3502.665686	502336.570527	49.554804
3502.679237	502346.994348	49.559809
3502.786125	502347.888570	49.564813
3502.913844	502345.439182	49.569818
3502.715125	502354.732499	49.574823
3502.849942	502346.917238	49.579828
3502.506368	502352.488246	49.584833
3502.543701	502347.168325	49.589837
3502.850536	502353.598139	49.594842
3502.770410	502359.481781	49.599847
3502.890866	502348.379086	49.604852
3502.847569	502346.968946	49.609857
3502.845458	502351.321934	49.614861
3502.888584	502356.882432	49.619866
3502.895761	502359.209516	49.624871
3502.982478	502345.328556	49.629876
3502.744492	502333.270287	49.634881
3502.931048	502324.738287	49.639885
3503.225511	502319.478939	49.644890
3502.982916	502315.670970	49.649895
3503.121194	502321.317661	49.654900
3503.010628	502325.131077	49.659905
3502.884182	502322.570025	49.664909
3503.170692	502306.531797	49.669914
3502.922281	502292.197653	49.674919
3503.418513	502274.810362	49.679924
3503.096347	502277.746233	49.684929
3502.922636	502273.876756	49.689933
3503.072849	502272.537246	49.694938
3502.973516	502270.427401	49.699943
3503.024496	502254.578185	49.704948
3503.149634	502234.162227	49.709953
3503.068375	502227.494512	49.714957
3503.066370	502224.711332	49.719962
3503.044529	502218.692168	49.724967
3503.375767	502215.097148	49.729972
3503.139883	502198.584664	49.734977
3502.710667	502188.074860	49.739981
3503.155597	502178.034223	49.744986
3502.790300	502194.641985	49.749991
3503.073926	502181.387721	49.754996
3503.023287	502179.371391	49.760001
3503.057051	502177.240498	49.765005
3502.816733	502161.740908	49.770010
3502.911377	502152.970294	49.775015
3502.992191	502143.594525	49.780020
3502.796292	502146.712906	49.785025
3503.063846	502138.471683	49.790029
3503.205362	502137.943321	49.795034
3502.875959	502148.674522	49.800039
3502.791129	502143.930574	49.805044
3502.945646	502138.288400	49.810049
3503.022888	502135.593904	49.815053
3502.932707	502101.546721	49.820058
3502.353410	502101.891459	49.825063
3502.887122	502098.416248	49.830068
3502.843249	502103.585684	49.835073
3502.794077	502102.834402	49.840077
3502.781465	502099.951656	49.845082
3502.540447	502097.560514	49.850087
3502.847778	502088.655030	49.855092
3502.688980	502098.650734	49.860097
3502.694555	502098.649973	49.865101
3503.176166	502100.244155	49.870106
3502.635094	502108.933760	49.875111
3502.800712	502098.836001	49.880116
3502.626920	502095.725672	49.885121
3502.820856	502096.302479	49.890125
3503.029509	502092.018247	49.895130
3502.808027	502099.341442	49.900135
3502.923320	502089.403467	49.905140
3502.757557	502070.956540	49.910145
3502.644646	502051.691453	49.915149
3502.793306	502053.338263	49.920154
3502.743124	502059.824613	49.925159
3502.735661	502051.677428	49.930164
3502.874689	502055.552676	49.935169
3502.923938	502058.176821	49.940173
3503.047336	502054.665230	49.945178
3502.695415	502053.860574	49.950183
3502.755077	502051.168844	49.955188
3502.956927	502058.779429	49.960193
3503.015336	502046.572894	49.965197
3502.980353	502040.808805	49.970202
3502.690471	502046.826928	49.975207
3503.048426	502042.063580	49.980212
3503.021187	502025.517957	49.985217
3502.814586	502009.658622	49.990221
3502.893478	502007.318128	49.995226
3503.274931	502014.191780	50.000231
3503.286780	502011.659436	50.005236
3502.783232	502012.953828	50.010241
3502.532060	502010.412444	50.015245
3502.906694	502008.278266	50.020250
3502.646964	502014.898976	50.025255
3502.976099	502004.977767	50.030260
3502.831825	501992.651394	50.035265
3502.392502	501973.994543	50.040269
3502.901976	501968.245601	50.045274
3503.015778	501974.199944	50.050279
3503.160337	501970.330709	50.055284
3502.874146	501971.388302	50.060289
3503.209344	501968.450561	50.065293
3503.122158	501966.642431	50.070298
3502.782252	501967.607290	50.075303
3502.672408	501972.230460	50.080308
3502.816898	501962.439635	50.085313
3502.829066	501949.278714	50.090317
3502.774161	501932.484317	50.095322
3502.681233	501925.109762	50.100327
3502.809608	501920.078996	50.105332
3502.792151	501923.270437	50.110337
3502.725194	501919.029724	50.115341
3502.962171	501912.412816	50.120346
3502.874324	501927.458613	50.125351
3502.961545	501920.106195	50.130356
3502.836202	501921.897550	50.135361
3502.660687	501914.738493	50.140365
3502.940618	501915.959672	50.145370
3502.730857	501924.546389	50.150375
3502.989138	501923.695894	50.155380
3502.613896	501923.350426	50.160385
3502.754304	501931.476898	50.165389
3502.902754	501916.320542	50.170394
3502.645373	501898.140976	50.175399
3502.800093	501888.702778	50.180404
3502.902080	501886.561067	50.185409
3502.877698	501883.123412	50.190413
3502.748627	501882.637810	50.195418
3502.811780	501880.046726	50.200423
3502.932581	501870.006534	50.205428
3502.840835	501880.497885	50.210433
3503.042151	501884.160877	50.215437
3502.812421	501878.933638	50.220442
3502.750496	501881.018646	50.225447
3502.860669	501884.544207	50.230452
3502.961467	501882.301459	50.235457
3502.714882	501868.371580	50.240461
3502.861724	501857.871754	50.245466
3502.836697	501853.826848	50.250471
3502.925623	501839.135345	50.255476
3502.445252	501843.361600	50.260481
3502.794720	501834.651777	50.265485
3502.906727	501832.862763	50.270490
3502.936478	501828.252457	50.275495
3502.892998	501832.510887	50.280500
3502.968748	501834.928427	50.285505
3502.998331	501835.328770	50.290509
3503.216506	501833.421750	50.295514
3502.927446	501824.559783	50.300519
3502.997155	501794.282664	50.305524
3503.030393	501804.045732	50.310529
3502.970268	501800.866772	50.315533
3503.148318	501791.272998	50.320538
3503.014115	501796.659250	50.325543
3502.761778	501798.420077	50.330548
3502.864226	501802.554224	50.335553
3502.904162	501796.778214	50.340557
3502.986245	501790.236354	50.345562
3502.796275	501766.934138	50.350567
3502.970663	501754.962134	50.355572
3502.896074	501752.139740	50.360577
3502.933051	501748.945423	50.365581
3502.838225	501748.251955	50.370586
3502.623080	501750.411808	50.375591
3502.613950	501741.303105	50.380596
3502.678048	501743.621274	50.385601
3502.868445	501740.048419	50.390605
3502.834810	501756.654783	50.395610
3503.007105	501755.463583	50.400615
3503.039487	501752.573669	50.405620
3502.800538	501756.559336	50.410625
3502.451820	501763.902780	50.415629
3503.021116	501749.945079	50.420634
3502.567624	501738.173528	50.425639
3502.736696	501725.696218	50.430644
3502.963451	501713.007332	50.435649
3502.868985	501712.718707	50.440653
3502.738244	501703.983494	50.445658
3502.264203	501714.788430	50.450663
3502.730551	501704.946592	50.455668
3502.573959	501711.601726	50.460673
3502.779013	501702.307312	50.465677
3502.719470	501707.125051	50.470682
3502.665345	501719.584446	50.475687
3502.792543	501705.241072	50.480692
3502.529935	501712.419089	50.485697
3502.534288	501718.390817	50.490701
3502.637959	501711.794904	50.495706
3502.730645	501720.890656	50.500711
3502.681729	501712.142515	50.505716
3502.605317	501716.203727	50.510721
3502.394769	501707.278679	50.515725
3502.717354	501701.255514	50.520730
3502.892517	501703.961035	50.525735
3502.889062	501677.693685	50.530740
3502.755557	501656.659974	50.535745
3502.589190	501619.789585	50.540749
3502.793781	501563.323837	50.545754
3502.301298	501499.983450	50.550759
3502.666368	501417.223552	50.555764
3502.619285	501334.680253	50.560769
3502.018060	501237.950999	50.565773
3502.125500	501124.507704	50.570778
3501.947717	501018.700968	50.575783
3501.627389	500896.162568	50.580788
3501.529899	500766.350103	50.585793
3501.516316	500618.149899	50.590797
3501.484978	500474.658575	50.595802
3501.072499	500320.546226	50.600807
3501.062701	500153.613384	50.605812
3500.735360	499972.910559	50.610817
3500.421070	499797.164418	50.615821
3500.743272	499599.904249	50.620826
3500.193353	499407.386100	50.625831
3500.145562	499188.008625	50.630836
3499.573356	498974.735187	50.635841
3499.391191	498750.665891	50.640845
3499.223693	498507.861428	50.645850
3498.792497	498285.749318	50.650855
3498.782061	498031.017318	50.655860
3498.473356	497783.416194	50.660865
3498.043751	497515.783457	50.665869
3497.757737	497261.387883	50.670874
3497.184377	496979.189823	50.675879
3497.331087	496699.404890	50.680884
3496.877173	496416.622283	50.685889
3496.630641	496115.728126	50.690893
3496.312363	495820.510808	50.695898
3495.467844	495519.296256	50.700903
3495.453951	495196.579143	50.705908
3495.226965	494879.712675	50.710913
3494.780703	494557.457658	50.715917
3494.638968	494218.895402	50.720922
3493.784545	493884.844755	50.725927
3493.495894	493539.052407	50.730932
3492.770362	493196.765894	50.735937
3492.443695	492848.029642	50.740941
3492.487044	492488.999333	50.745946
3491.800825	492132.811895	50.750951
3491.271737	491761.096773	50.755956
3490.798873	491394.226894	50.760961
3490.379081	491025.568887	50.765965
3490.024819	490644.485550	50.770970
3489.769287	490255.832768	50.775975
3489.227238	489856.227071	50.780980
3488.522969	489464.032902	50.785985
3488.001517	489068.104334	50.790989
3487.812826	488665.682409	50.795994
3487.092788	488258.726711	50.800999
3486.683242	487847.002594	50.806004
3486.196257	487440.397611	50.811009
3485.402911	487013.621644	50.816013
3485.223594	486593.526709	50.821018
3484.382623	486176.161159	50.826023
3484.301216	485741.493774	50.831028
3483.690741	485314.397476	50.836033
3483.032053	484875.090436	50.841037
3482.737790	484438.350045	50.846042
3481.865232	483995.662428	50.851047
3481.125922	483548.890559	50.856052
3480.985466	483104.496196	50.861057
3480.338271	482644.009621	50.866061
3479.727484	482195.564865	50.871066
3479.094963	481738.854421	50.876071
3478.730292	481270.943855	50.881076
3477.655390	480822.692812	50.886081
3476.963611	480360.385778	50.891085
3476.756344	479898.700652	50.896090
3476.168277	479437.115535	50.901095
3475.602889	478966.850679	50.906100
3475.018244	478504.533724	50.911105
3474.214383	478030.787649	50.916109
3473.595178	477553.656306	50.921114
3472.883116	477082.204253	50.926119
3472.617396	476592.476195	50.931124
3471.720982	476126.200078	50.936129
3471.034800	475648.526897	50.941133
3470.842346	475166.658881	50.946138
3470.316815	474686.149785	50.951143
3469.419112	474199.048127	50.956148
3468.789759	473720.559906	50.961153
3468.187396	473235.415862	50.966157
3467.688534	472755.414258	50.971162
3466.934667	472261.501522	50.976167
3466.596867	471764.722967	50.981172
3465.810051	471274.796298	50.986177
3464.926215	470770.881430	50.991181
3464.425046	470273.180059	50.996186
3463.568137	469782.367068	51.001191
3462.691054	469287.591109	51.006196
3462.194988	468796.444197	51.011201
3461.436151	468302.538652	51.016205
3461.033524	467808.007359	51.021210
3460.074718	467326.177442	51.026215
3459.396420	466823.097544	51.031220
3458.853920	466325.967418	51.036225
3458.013684	465834.703927	51.041229
3457.541554	465338.401401	51.046234
3456.420036	464847.108703	51.051239
3456.288414	464357.473722	51.056244
3455.494214	463859.564770	51.061249
3454.663927	463354.550080	51.066253
3453.942742	462864.872606	51.071258
3453.161220	462382.648633	51.076263
3452.894911	461884.153852	51.081268
3451.794870	461384.815707	51.086273
3451.314736	460898.808505	51.091277
3451.095239	460398.801223	51.096282
3450.085303	459903.675176	51.101287
3449.231768	459396.897755	51.106292
3448.233343	458914.783062	51.111297
3447.936886	458416.061319	51.116301
3447.262560	457920.127177	51.121306
3446.640854	457429.398414	51.126311
3446.096688	456924.493392	51.131316
3445.071529	456430.661117	51.136321
3444.098878	455935.236921	51.141325
3443.433690	455445.790129	51.146330
3442.778715	454950.699693	51.151335
3442.074743	454462.049223	51.156340
3441.286435	453980.149163	51.161345
3440.475511	453482.463545	51.166349
3440.039071	452993.434500	51.171354
3439.362778	452517.066564	51.176359
3438.627961	452028.622001	51.181364
3437.873289	451540.170099	51.186369
3437.054622	451059.024596	51.191373
3436.448778	450570.376226	51.196378
3435.749389	450090.713815	51.201383
3434.892326	449605.991901	51.206388
3434.208465	449127.220391	51.211393
3433.493617	448644.079682	51.216397
3432.964992	448163.944332	51.221402
3431.949986	447688.240354	51.226407
3431.316283	447199.728246	51.231412
3430.576586	446726.397157	51.236417
3429.894104	446253.199736	51.241421
3429.228102	445781.969556	51.246426
3428.554064	445302.965924	51.251431
3427.858133	444821.976629	51.256436
3426.992133	444358.210682	51.261441
3426.619087	443874.968690	51.266445
3425.937958	443401.358851	51.271450
3425.005848	442929.758917	51.276455
3424.227651	442444.521767	51.281460
3423.466044	441979.779582	51.286465
3422.627476	441510.319779	51.291469
3422.019390	441048.378088	51.296474
3421.310481	440595.377960	51.301479
3420.722807	440111.079219	51.306484
3419.775277	439644.240395	51.311489
3418.935174	439195.854732	51.316493
3418.657237	438721.912093	51.321498
3417.467691	438267.624956	51.326503
3417.031747	437804.376441	51.331508
3416.274522	437342.287011	51.336513
3415.323886	436885.296699	51.341517
3414.640965	436432.926727	51.346522
3413.931974	435976.033879	51.351527
3413.582477	435515.521680	51.356532
3412.865106	435075.775408	51.361537
3411.902541	434605.873961	51.366541
3411.328851	434145.169075	51.371546
3410.726124	433697.738793	51.376551
3409.741702	433243.251975	51.381556
3409.075795	432788.935207	51.386561
3408.651260	432335.410085	51.391565
3407.697533	431891.786801	51.396570
3406.982197	431432.248732	51.401575
3406.333318	430987.012812	51.406580
3405.285796	430536.982387	51.411585
3404.318224	430100.135578	51.416589
3403.886090	429658.803816	51.421594
3402.843056	429223.553993	51.426599
3402.375806	428777.159634	51.431604
3401.524274	428345.089945	51.436609
3400.956237	427904.131039	51.441613
3400.536996	427473.070674	51.446618
3399.726839	427043.588822	51.451623
3399.517096	426594.755081	51.456628
3398.390860	426157.055247	51.461633
3397.635031	425708.953241	51.466637
3397.012226	425269.305326	51.471642
3396.060035	424841.918479	51.476647
3395.620237	424404.360883	51.481652
3395.001444	423979.879220	51.486657
3394.358384	423550.365807	51.491661
3393.148673	423111.918527	51.496666
3392.327812	422687.677223	51.501671
3392.145986	422250.120359	51.506676
3391.407654	421825.954253	51.511681
3390.225524	421399.616516	51.516685
3389.745576	420963.407154	51.521690
3388.934396	420543.551025	51.526695
3388.316304	420104.784439	51.531700
3387.695559	419693.166355	51.536705
3387.204316	419275.679124	51.541709
3386.441250	418841.869115	51.546714
3385.492762	418417.912833	51.551719
3385.024477	417994.483929	51.556724
3383.974311	417579.879709	51.561729
3383.239705	417154.295580	51.566733
3382.896405	416729.633995	51.571738
3382.381777	416321.659032	51.576743
3381.637535	415890.747854	51.581748
3380.603289	415467.599484	51.586753
3380.118528	415047.965710	51.591757
3379.441550	414631.074747	51.596762
3378.587726	414208.844834	51.601767
3378.035204	413794.361235	51.606772
3377.370449	413376.078301	51.611777
3376.194190	412969.303948	51.616781
3375.762928	412539.589245	51.621786
3374.930613	412134.857841	51.626791
3374.306220	411722.592260	51.631796
3373.441229	411317.041705	51.636801
3372.867433	410907.297726	51.641805
3372.109582	410489.217201	51.646810
3371.506498	410096.313741	51.651815
3371.003708	409679.706190	51.656820
3370.049316	409275.082197	51.661825
3369.156439	408865.614808	51.666829
3368.626531	408459.718392	51.671834
3367.859727	408054.311416	51.676839
3367.426023	407652.124598	51.681844
3366.372453	407245.202000	51.686849
3365.838015	406850.949423	51.691853
3365.006335	406455.849294	51.696858
3364.416627	406061.442831	51.701863
3363.967734	405656.970373	51.706868
3363.299430	405258.804754	51.711873
3362.202468	404861.972557	51.716877
3361.693203	404454.952466	51.721882
3361.056190	404058.799770	51.726887
3360.640639	403662.734120	51.731892
3359.580226	403260.284281	51.736897
3358.730552	402862.142223	51.741901
3358.379964	402454.740697	51.746906
3357.359525	402069.019149	51.751911
3356.900425	401662.031287	51.756916
3356.164593	401280.779522	51.761921
3355.425220	400883.688215	51.766925
3354.610160	400487.620704	51.771930
3353.828040	400097.694477	51.776935
3353.307658	399706.654547	51.781940
3352.602747	399323.874985	51.786945
3351.871292	398935.096047	51.791949
3351.664733	398536.849461	51.796954
3350.712314	398159.941989	51.801959
3350.078969	397765.642832	51.806964
3349.222510	397371.272549	51.811969
3348.385685	396981.673650	51.816973
3347.711162	396592.171611	51.821978
3347.172105	396202.262256	51.826983
3346.770954	395808.564052	51.831988
3345.829862	395433.250773	51.836993
3345.113358	395044.703372	51.841997
3344.669975	394657.074371	51.847002
3343.721157	394274.503822	51.852007
3343.161991	393868.884372	51.857012
3342.545595	393492.049021	51.862017
3341.815045	393108.363022	51.867021
3341.265949	392715.999698	51.872026
3340.417223	392333.467812	51.877031
3340.119749	391941.030428	51.882036
3338.963197	391560.191273	51.887041
3338.262421	391176.707868	51.892045
3337.717837	390780.711412	51.897050
3337.122935	390409.992059	51.902055
3336.464376	390020.183572	51.907060
3335.618484	389634.061837	51.912065
3334.784933	389252.993897	51.917069
3334.528358	388871.754325	51.922074
3333.589751	388492.551010	51.927079
3333.107873	388098.777557	51.932084
3332.336718	387726.405131	51.937089
3331.231097	387339.129840	51.942093
3331.178403	386953.209586	51.947098
3330.069836	386574.852001	51.952103
3329.290438	386192.217161	51.957108
3328.882042	385816.614439	51.962113
3328.123421	385442.716165	51.967117
3327.490346	385057.452443	51.972122
3326.585260	384680.746828	51.977127
3326.481705	384301.952453	51.982132
3325.300785	383930.114591	51.987137
3324.536803	383558.054476	51.992141
3324.023586	383176.083650	51.997146
3323.029649	382805.858014	52.002151
3322.256628	382433.279491	52.007156
3321.776704	382062.609191	52.012161
3320.978058	381678.862595	52.017165
3320.437797	381303.718312	52.022170
3319.644695	380942.293151	52.027175
3319.229957	380562.772710	52.032180
3318.421714	380191.703720	52.037185
3317.580615	379831.496455	52.042189
3317.439507	379448.869709	52.047194
3316.269043	379090.793189	52.052199
3315.757462	378715.288441	52.057204
3315.027167	378345.486555	52.062209
3314.271605	377982.959498	52.067213
3313.759595	377612.556604	52.072218
3312.921989	377249.654232	52.077223
3311.898908	376865.844490	52.082228
3311.493418	376499.280500	52.087233
3311.024724	376130.688256	52.092237
3310.534845	375761.282004	52.097242
3309.771308	375404.252273	52.102247
3308.919080	375030.012816	52.107252
3308.502632	374662.670666	52.112257
3307.382138	374291.392037	52.117261
3306.876217	373913.729807	52.122266
3305.831881	373560.009649	52.127271
3305.486264	373191.396596	52.132276
3304.694762	372830.278649	52.137281
3303.919921	372472.410999	52.142285
3303.399524	372106.588666	52.147290
3302.680364	371751.402467	52.152295
3302.227803	371385.664830	52.157300
3301.487299	371017.578266	52.162305
3300.783303	370662.227800	52.167309
3300.143149	370288.954820	52.172314
3299.126217	369931.485347	52.177319
3298.655376	369569.423628	52.182324
3298.291753	369200.930958	52.187329
3297.232922	368858.875876	52.192333
3296.896881	368483.096734	52.197338
3295.853739	368123.937249	52.202343
3295.446202	367759.662380	52.207348
3294.740764	367400.239972	52.212353
3294.096476	367049.124289	52.217357
3293.289116	366680.858472	52.222362
3292.470030	366326.889757	52.227367
3291.599833	365961.451920	52.232372
3291.306713	365603.908677	52.237377
3290.538320	365250.686628	52.242381
3289.796490	364884.125625	52.247386
3289.110469	364530.477790	52.252391
3288.760118	364166.316982	52.257396
3288.267311	363808.205837	52.262401
3287.503110	363448.989838	52.267405
3286.742424	363080.661613	52.272410
3285.763950	362734.755499	52.277415
3285.362707	362367.357013	52.282420
3284.918548	362005.814579	52.287425
3283.828014	361650.630905	52.292429
3283.249582	361280.860057	52.297434
3282.670876	360927.014825	52.302439
3281.756720	360565.357457	52.307444
3281.017486	360215.857929	52.312449
3280.096847	359850.124870	52.317453
3279.667435	359495.710954	52.322458
3278.720752	359153.004966	52.327463
3278.378935	358793.711843	52.332468
3277.508297	358444.016562	52.337473
3276.925296	358103.383061	52.342477
3276.311816	357744.074215	52.347482
3275.346056	357398.050750	52.352487
3274.996020	357036.048567	52.357492
3274.157466	356693.791609	52.362497
3273.463866	356346.750708	52.367501
3272.821093	355991.047200	52.372506
3272.101246	355645.506954	52.377511
3271.081611	355296.067326	52.382516
3270.491688	354945.106763	52.387521
3269.850822	354601.735374	52.392525
3269.535101	354258.335678	52.397530
3268.663753	353921.230987	52.402535
3268.073412	353572.195088	52.407540
3267.185873	353228.955266	52.412545
3266.521782	352890.436784	52.417549
3266.279628	352534.620243	52.422554
3264.925304	352194.094109	52.427559
3264.573040	351852.312927	52.432564
3264.056279	351509.842945	52.437569
3263.004542	351168.676951	52.442573
3262.610261	350822.238409	52.447578
3261.943637	350485.079107	52.452583
3261.321993	350140.835365	52.457588
3260.508169	349786.286901	52.462593
3259.857328	349444.537470	52.467597
3259.457172	349107.658243	52.472602
3258.562912	348765.866689	52.477607
3257.896776	348422.637099	52.482612
3257.306602	348086.748778	52.487617
3256.362371	347746.358601	52.492621
3255.922921	347395.018642	52.497626
3254.921892	347059.723566	52.502631
3254.644381	346717.058233	52.507636
3253.476808	346385.475998	52.512641
3252.896299	346052.704508	52.517645
3252.493371	345700.151918	52.522650
3251.607482	345367.602888	52.527655
3251.166413	345034.574323	52.532660
3250.566365	344688.409856	52.537665
3249.803048	344349.217811	52.542669
3249.304179	344014.258082	52.547674
3248.216859	343676.004225	52.552679
3247.559338	343335.338714	52.557684
3247.114236	342992.321358	52.562689
3246.318828	342663.204255	52.567693
3245.706046	342321.202241	52.572698
3244.951487	341989.045947	52.577703
3244.339276	341649.356325	52.582708
3243.675477	341317.614694	52.587713
3242.818414	340976.941860	52.592717
3242.322605	340642.471805	52.597722
3241.622291	340316.101420	52.602727
3241.149925	339968.896636	52.607732
3240.534152	339639.072897	52.612737
3239.552497	339292.377626	52.617741
3239.240471	338954.662043	52.622746
3238.277296	338635.655547	52.627751
3237.426741	338290.257696	52.632756
3236.773460	337962.900290	52.637761
3236.184295	337629.498040	52.642765
3235.776847	337285.195630	52.647770
3234.632460	336962.467424	52.652775
3234.091805	336623.273779	52.657780
3233.415925	336287.179978	52.662785
3232.983934	335970.596431	52.667789
3232.463958	335626.023049	52.672794
3231.959144	335295.803064	52.677799
3231.061943	334955.384411	52.682804
3230.180694	334620.536580	52.687809
3229.704637	334291.045351	52.692813
3228.934472	333950.474242	52.697818
3228.380920	333623.919619	52.702823
3227.693294	333281.651938	52.707828
3227.265845	332950.644571	52.712833
3225.986283	332618.446619	52.717837
3225.524527	332286.932365	52.722842
3224.905510	331954.601310	52.727847
3224.496648	331611.899468	52.732852
3223.456267	331285.487282	52.737857
3222.564477	330959.126472	52.742861
3222.160282	330622.656427	52.747866
3221.432855	330299.652596	52.752871
3220.670904	329963.185164	52.757876
3220.296749	329638.773210	52.762881
3219.343533	329310.021582	52.767885
3219.089189	328973.596614	52.772890
3218.357660	328644.195949	52.777895
3217.678611	328309.922820	52.782900
3216.417950	327986.585892	52.787905
3216.133720	327652.451070	52.792909
3215.585975	327327.343692	52.797914
3214.429134	327002.331292	52.802919
3214.150039	326673.079645	52.807924
3213.622187	326342.516581	52.812929
3212.687779	326014.460592	52.817933
3211.873502	325684.652944	52.822938
3211.230210	325366.477640	52.827943
3210.674151	325029.981313	52.832948
3209.991028	324707.659657	52.837953
3209.331690	324385.358411	52.842957
3208.764053	324049.980090	52.847962
3207.944478	323734.575980	52.852967
3207.462233	323402.007637	52.857972
3206.867331	323081.396944	52.862977
3205.920468	322750.809064	52.867981
3205.528840	322410.609588	52.872986
3204.896345	322095.118757	52.877991
3204.093661	321766.821185	52.882996
3203.572055	321438.274197	52.888001
3202.819412	321113.225270	52.893005
3201.981646	320774.235641	52.898010
3201.162071	320462.714981	52.903015
3200.503992	320132.911576	52.908020
3200.131036	319811.260560	52.913025
3199.181688	319493.391557	52.918029
3198.875740	319161.288203	52.923034
3198.120028	318833.990745	52.928039
3197.416239	318493.800007	52.933044
3196.936857	318181.020899	52.938049
3196.148765	317847.792331	52.943053
3195.404505	317515.192201	52.948058
3194.697467	317190.707574	52.953063
3193.792534	316870.123470	52.958068
3192.918543	316546.936193	52.963073
3192.223335	316236.170878	52.968077
3191.805207	315912.832969	52.973082
3191.092012	315609.732841	52.978087
3190.135734	315272.142279	52.983092
3189.416608	314969.193902	52.988097
3188.668675	314648.246641	52.993101
3188.391659	314329.286384	52.998106
3187.599910	314021.941488	53.003111
3187.341469	313702.034182	53.008116
3186.949284	313378.633070	53.013121
3185.698648	313060.917843	53.018125
3185.256331	312735.078157	53.023130
3184.924061	312411.333552	53.028135
3183.833871	312086.409215	53.033140
3183.323347	311776.670564	53.038145
3182.500571	311455.699862	53.043149
3182.023800	311126.448567	53.048154
3181.156219	310807.622044	53.053159
3180.344239	310488.658488	53.058164
3179.952411	310169.194658	53.063169
3179.225639	309852.660396	53.068173
3178.578437	309524.959230	53.073178
3177.377493	309210.509909	53.078183
3177.095831	308890.439403	53.083188
3176.507671	308582.053875	53.088193
3175.670120	308260.796374	53.093197
3175.329133	307938.313530	53.098202
3174.516767	307628.229405	53.103207
3173.825523	307317.361379	53.108212
3173.225223	306993.261837	53.113217
3172.675418	306674.221010	53.118221
3172.161886	306352.703513	53.123226
3171.095866	306031.832846	53.128231
3170.576197	305707.615377	53.133236
3169.700824	305394.428931	53.138241
3168.614380	305074.195748	53.143245
3168.128580	304746.099791	53.148250
3167.397326	304449.771894	53.153255
3166.841464	304131.744392	53.158260
3166.350340	303828.170383	53.163265
3165.419714	303513.409405	53.168269
3165.069016	303201.917436	53.173274
3164.181493	302896.468709	53.178279
3163.637553	302571.789172	53.183284
3163.051229	302263.286461	53.188289
3161.902987	301953.344042	53.193293
3161.444241	301639.319176	53.198298
3160.667003	301336.880167	53.203303
3159.842239	301026.171577	53.208308
3158.988000	300716.511127	53.213313
3158.576532	300418.749122	53.218317
3157.978915	300109.072315	53.223322
3157.088965	299823.201231	53.228327
3156.956398	299500.512756	53.233332
3156.182893	299196.897529	53.238337
3155.500309	298886.391403	53.243341
3155.075555	298582.235992	53.248346
3154.060141	298263.351941	53.253351
3153.547583	297956.331566	53.258356
3152.942396	297653.119828	53.263361
3152.110201	297333.542921	53.268365
3151.445656	297030.517759	53.273370
3150.734653	296716.344977	53.278375
3150.223762	296414.415000	53.283380
3149.474849	296110.917772	53.288385
3148.679948	295806.943452	53.293389
3148.221273	295487.864468	53.298394
3147.442602	295191.552146	53.303399
3146.731273	294879.184481	53.308404
3146.081561	294571.441577	53.313409
3145.782303	294263.057003	53.318413
3144.913732	293952.546398	53.323418
3143.961761	293651.471381	53.328423
3143.495000	293340.259600	53.333428
3142.943815	293042.558372	53.338433
3142.083835	292734.871475	53.343437
3141.519461	292415.447863	53.348442
3140.741445	292116.329628	53.353447
3140.513465	291802.378336	53.358452
3139.357542	291496.875832	53.363457
3138.869116	291188.822433	53.368461
3138.255543	290888.352288	53.373466
3137.381462	290582.498407	53.378471
3136.823095	290273.614485	53.383476
3136.214656	289963.490195	53.388481
3135.389393	289663.968907	53.393485
3134.783882	289347.527445	53.398490
3133.820661	289047.212323	53.403495
3133.374841	288745.439743	53.408500
3132.766765	288437.962268	53.413505
3132.084671	288136.455631	53.418509
3131.573607	287829.267766	53.423514
3130.607501	287538.425528	53.428519
3129.946256	287221.786774	53.433524
3129.444719	286921.039849	53.438529
3128.509423	286626.524507	53.443533
3128.002473	286321.983160	53.448538
3127.379838	286027.137660	53.453543
3126.601905	285714.794518	53.458548
3126.210459	285419.810046	53.463553
3125.170318	285115.453880	53.468557
3124.683397	284807.138783	53.473562
3123.900181	284518.633528	53.478567
3123.128079	284203.817785	53.483572
3122.680906	283914.927831	53.488577
3122.060254	283621.557272	53.493581
3121.159571	283316.413614	53.498586
3120.574493	283008.341904	53.503591
3120.041952	282692.086394	53.508596
3119.363969	282392.076915	53.513601
3118.543078	282091.835184	53.518605
3118.360129	281786.245877	53.523610
3117.272392	281490.299214	53.528615
3116.577496	281186.242266	53.533620
3115.835990	280888.355848	53.538625
3114.878917	280590.376053	53.543629
3114.435669	280286.126017	53.548634
3113.538304	280002.602477	53.553639
3113.065844	279709.129885	53.558644
3112.490463	279421.200081	53.563649
3111.389322	279122.274652	53.568653
3111.361636	278822.236916	53.573658
3110.530331	278536.613976	53.578663
3110.085943	278234.757325	53.583668
3109.341583	277930.528556	53.588673
3108.392580	277643.166665	53.593677
3107.841924	277338.041155	53.598682
3107.038196	277048.593194	53.603687
3106.475387	276746.729420	53.608692
3105.890965	276450.446579	53.613697
3105.114857	276162.776865	53.618701
3104.681837	275862.063940	53.623706
3104.007374	275571.423727	53.628711
3103.189594	275269.192577	53.633716
3102.626869	274975.452948	53.638721
3101.686937	274678.232886	53.643725
3101.213926	274378.111930	53.648730
3100.456334	274088.350700	53.653735
3099.585732	273792.902433	53.658740
3099.058774	273503.766888	53.663745
3098.307253	273214.310334	53.668749
3098.276387	272901.436178	53.673754
3097.144088	272622.150873	53.678759
3096.675620	272322.767864	53.683764
3095.871199	272026.927226	53.688769
3095.055845	271736.920619	53.693773
3094.378518	271435.558792	53.698778
3093.631652	271149.845604	53.703783
3093.158507	270865.158829	53.708788
3092.336806	270574.695023	53.713793
3091.419754	270284.653872	53.718797
3090.915089	269994.038171	53.723802
3090.410713	269706.147620	53.728807
3089.730129	269412.299985	53.733812
3089.100904	269113.299721	53.738817
3088.694059	268822.337826	53.743821
3087.947253	268533.441835	53.748826
3087.083696	268242.017604	53.753831
3086.666459	267942.805973	53.758836
3085.793865	267662.563992	53.763841
3084.781226	267372.131527	53.768845
3084.589480	267072.451659	53.773850
3083.880396	266785.205906	53.778855
3083.088948	266497.667715	53.783860
3082.092544	266204.788323	53.788865
3081.435950	265915.115247	53.793869
3080.858037	265619.954228	53.798874
3079.985590	265343.355351	53.803879
3079.759219	265055.728558	53.808884
3078.923026	264769.701076	53.813889
3077.890859	264484.952731	53.818893
3077.350320	264195.109558	53.823898
3076.787861	263919.532178	53.828903
3076.423413	263630.756663	53.833908
3075.791724	263345.105288	53.838913
3075.101599	263061.449879	53.843917
3074.510809	262770.698862	53.848922
3073.504554	262496.033188	53.853927
3072.788187	262200.361722	53.858932
3072.210402	261910.144183	53.863937
3071.633822	261632.635191	53.868941
3071.285269	261341.923445	53.873946
3070.375430	261064.620488	53.878951
3069.575913	260771.153701	53.883956
3069.161332	260487.635127	53.888961
3068.208479	260204.151072	53.893965
3067.886286	259914.582553	53.898970
3066.784911	259633.159980	53.903975
3066.450430	259340.741598	53.908980
3065.947077	259048.986943	53.913985
3065.016554	258771.511163	53.918989
3064.783397	258470.240399	53.923994
3063.696489	258177.687684	53.928999
3063.124721	257886.021540	53.934004
3062.377435	257607.626638	53.939009
3061.661718	257324.362754	53.944013
3061.111716	257021.845016	53.949018
3060.102562	256754.927434	53.954023
3059.535685	256469.781877	53.959028
3059.041724	256187.859489	53.964033
3058.042461	255905.355270	53.969037
3057.880229	255612.251856	53.974042
3057.193847	255335.123381	53.979047
3056.331155	255039.635794	53.984052
3055.628510	254765.057349	53.989057
3054.926992	254486.251526	53.994061
3054.637970	254190.725263	53.999066
3053.762556	253905.071609	54.004071
3052.907172	253623.820995	54.009076
3052.293286	253343.016429	54.014081
3051.213057	253060.121374	54.019085
3050.586960	252775.728704	54.024090
3049.749125	252507.719746	54.029095
3049.293860	252227.884904	54.034100
3048.571890	251949.187767	54.039105
3047.717728	251684.467799	54.044109
3047.273329	251404.607015	54.049114
3046.575446	251143.122851	54.054119
3046.133597	250861.301571	54.059124
3045.569538	250588.438888	54.064129
3044.522095	250308.395147	54.069133
3043.892983	250028.005519	54.074138
3043.076391	249754.420129	54.079143
3042.765615	249474.872363	54.084148
3042.027432	249208.813544	54.089153
3041.285009	248938.451999	54.094157
3040.933826	248651.297565	54.099162
3039.787406	248384.871779	54.104167
3039.239140	248108.980168	54.109172
3038.635711	247827.622527	54.114177
3038.139868	247562.623136	54.119181
3037.464948	247287.287816	54.124186
3036.801293	247020.151299	54.129191
3036.224290	246732.883343	54.134196
3035.351926	246460.534844	54.139201
3034.482352	246191.547913	54.144205
3034.118739	245913.797511	54.149210
3033.490115	245638.457912	54.154215
3032.705957	245363.856502	54.159220
3032.255688	245087.954950	54.164225
3031.407227	244816.700795	54.169229
3030.772451	244538.079227	54.174234
3029.859223	244276.564267	54.179239
3029.268016	243990.042566	54.184244
3028.606491	243714.711964	54.189249
3027.982714	243446.608146	54.194253
3027.654376	243174.816547	54.199258
3026.530149	242902.769501	54.204263
3025.710611	242640.809990	54.209268
3025.569358	242355.213739	54.214273
3024.777036	242084.236342	54.219277
3024.492728	241802.585605	54.224282
3023.688316	241536.678854	54.229287
3022.933749	241260.298642	54.234292
3022.247068	240982.736908	54.239297
3021.425214	240704.764290	54.244301
3021.260747	240425.313144	54.249306
3020.551935	240154.148473	54.254311
3019.498654	239875.756016	54.259316
3019.106973	239598.329003	54.264321
3017.938834	239320.337995	54.269325
3017.326099	239041.292079	54.274330
3016.441987	238783.832767	54.279335
3016.161917	238506.543457	54.284340
3015.480157	238236.754003	54.289345
3014.845789	237971.566731	54.294349
3014.160862	237687.646374	54.299354
3013.478831	237420.812763	54.304359
3012.809535	237146.058423	54.309364
3012.085244	236871.288006	54.314369
3011.565528	236596.587749	54.319373
3010.957036	236316.860373	54.324378
3010.099494	236057.111372	54.329383
3009.595538	235776.859570	54.334388
3009.092341	235501.777528	54.339393
3007.965735	235235.528929	54.344397
3007.593053	234958.441473	54.349402
3006.704856	234687.725855	54.354407
3005.832929	234421.413554	54.359412
3005.405841	234154.165770	54.364417
3004.549307	233882.225010	54.369421
3004.206550	233607.173518	54.374426
3003.080366	233342.890416	54.379431
3002.649504	233078.854431	54.384436
3002.339270	232805.047683	54.389441
3001.192600	232540.897267	54.394445
3000.650267	232263.309307	54.399450
3000.060460	232004.623111	54.404455
2999.458532	231731.476641	54.409460
2998.589997	231455.699559	54.414465
2997.914667	231179.510747	54.419469
2997.642045	230919.453200	54.424474
2996.414269	230653.894883	54.429479
2995.928428	230386.717585	54.434484
2995.303647	230124.248122	54.439489
2994.421588	229861.438191	54.444493
2994.181718	229591.550697	54.449498
2993.150364	229326.423400	54.454503
2992.841359	229062.175547	54.459508
2991.940561	228803.802021	54.464513
2991.662682	228535.960632	54.469517
2991.109678	228258.844551	54.474522
2989.925907	227993.643450	54.479527
2988.971981	227722.372332	54.484532
2988.834417	227458.484001	54.489537
2987.956315	227194.815537	54.494541
2987.204313	226927.588763	54.499546
2986.758139	226671.721108	54.504551
2985.866185	226408.235460	54.509556
2985.352417	226142.424702	54.514561
2984.713328	225877.118375	54.519565
2984.135593	225602.815401	54.524570
2983.022626	225344.078338	54.529575
2982.423713	225073.472290	54.534580
2981.974095	224817.177940	54.539585
2981.050121	224558.082408	54.544589
2980.433924	224290.957042	54.549594
2979.919481	224025.585950	54.554599
2979.277680	223783.379494	54.559604
2978.439942	223516.750021	54.564609
2977.932522	223253.378983	54.569613
2977.570455	222986.294058	54.574618
2976.780660	222727.845090	54.579623
2976.039310	222460.389144	54.584628
2975.577331	222188.154312	54.589633
2974.757934	221929.763556	54.594637
2973.940649	221662.500560	54.599642
2973.214062	221400.481563	54.604647
2972.885201	221141.188323	54.609652
2972.197210	220888.241325	54.614657
2970.996391	220632.142987	54.619661
2970.853499	220356.197900	54.624666
2970.197646	220093.713893	54.629671
2969.154122	219832.234160	54.634676
2968.620914	219568.879678	54.639681
2967.816766	219313.346757	54.644685
2967.213814	219040.801725	54.649690
2966.266470	218781.334430	54.654695
2965.994045	218523.046869	54.659700
2965.231374	218274.130252	54.664705
2964.587782	218007.641915	54.669709
2963.895938	217747.997805	54.674714
2962.768911	217496.366548	54.679719
2962.488296	217233.464148	54.684724
2961.862872	216976.714546	54.689729
2960.991450	216717.789951	54.694733
2960.477041	216461.368313	54.699738
2959.716393	216208.818009	54.704743
2958.945563	215957.186705	54.709748
2958.371253	215704.443235	54.714753
2957.955021	215448.238861	54.719757
2957.367231	215182.477802	54.724762
2956.357924	214928.673148	54.729767
2955.723505	214669.833153	54.734772
2955.466636	214416.433140	54.739777
2954.302524	214158.646310	54.744781
2954.044363	213901.531657	54.749786
2953.184990	213645.276869	54.754791
2952.513916	213384.576465	54.759796
2951.871461	213133.533408	54.764801
2951.140991	212878.903097	54.769805
2950.863634	212611.130037	54.774810
2949.907033	212367.178358	54.779815
2948.855214	212107.841503	54.784820
2948.409626	211851.375355	54.789825
2947.761362	211600.339021	54.794829
2947.084323	211342.422319	54.799834
2946.106198	211097.053225	54.804839
2945.390772	210837.362681	54.809844
2945.094179	210587.407373	54.814849
2944.395357	210346.744427	54.819853
2944.265444	210087.842434	54.824858
2943.343434	209835.112587	54.829863
2942.440309	209573.344071	54.834868
2941.916233	209322.258782	54.839873
2941.190029	209059.382533	54.844877
2940.976828	208806.786405	54.849882
2939.987740	208558.552398	54.854887
2939.423980	208293.782703	54.859892
2938.891027	208046.076716	54.864897
2937.801739	207790.670657	54.869901
2937.494213	207522.618218	54.874906
2936.646289	207271.312478	54.879911
2935.660320	207013.996934	54.884916
2934.915937	206762.956894	54.889921
2934.539182	206512.101502	54.894925
2934.010724	206256.994885	54.899930
2933.219101	206013.818019	54.904935
2932.584877	205751.755902	54.909940
2931.854228	205491.301060	54.914945
2931.078292	205250.250206	54.919949
2930.847036	204991.614784	54.924954
2929.925856	204744.747396	54.929959
2929.236964	204487.306591	54.934964
2928.258228	204228.601965	54.939969
2927.880558	203986.118757	54.944973
2927.248457	203734.144693	54.949978
2926.590580	203487.788166	54.954983
2925.878422	203222.097175	54.959988
2925.513131	202974.754759	54.964993
2924.640734	202728.499074	54.969997
2924.320032	202469.761762	54.975002
2923.482285	202213.296387	54.980007
2922.707832	201953.691527	54.985012
2922.365649	201700.382439	54.990017
2921.511222	201447.130139	54.995021
2921.274307	201180.711681	55.000026
2920.355886	200934.840137	55.005031
2919.764252	200667.054992	55.010036
2919.229223	200404.365198	55.015041
2918.237473	200149.117137	55.020045
2917.332535	199885.381241	55.025050
2916.563363	199637.404822	55.030055
2915.686123	199376.517512	55.035060
2915.299178	199131.766047	55.040065
2914.437937	198886.403605	55.045069
2913.902876	198626.331038	55.050074
2913.024198	198379.013953	55.055079
2912.062525	198124.966778	55.060084
2911.935591	197877.443895	55.065089
2911.106365	197637.872013	55.070093
2910.812822	197393.584474	55.075098
2910.017813	197140.037315	55.080103
2909.300038	196883.666932	55.085108
2908.586126	196639.118576	55.090113
2907.851122	196386.787116	55.095117
2907.786715	196134.757879	55.100122
2906.561751	195893.615069	55.105127
2905.736490	195633.590372	55.110132
2905.136598	195379.715424	55.115137
2904.543155	195143.833137	55.120141
2903.949693	194886.536699	55.125146
2903.130229	194646.149849	55.130151
2902.668896	194392.435959	55.135156
2902.151900	194144.839779	55.140161
2901.344657	193899.835594	55.145165
2900.960440	193635.908452	55.150170
2900.113080	193395.557356	55.155175
2898.897528	193144.068581	55.160180
2898.711069	192885.216366	55.165185
2897.780844	192646.803276	55.170189
2897.320670	192395.160470	55.175194
2896.944329	192145.821379	55.180199
2896.228619	191899.082008	55.185204
2895.692236	191644.325035	55.190209
2894.520489	191395.929966	55.195213
2894.073825	191141.504914	55.200218
2893.353331	190895.738295	55.205223
2892.751155	190647.333159	55.210228
2892.416816	190387.372293	55.215233
2891.452511	190138.861682	55.220237
2890.976488	189890.465873	55.225242
2890.124604	189645.108057	55.230247
2889.227190	189391.157926	55.235252
2888.598526	189141.924968	55.240257
2887.964536	188896.981764	55.245261
2887.645309	188633.707258	55.250266
2886.617212	188391.717130	55.255271
2885.783037	188144.812007	55.260276
2885.338800	187895.607241	55.265281
2884.714956	187648.569617	55.270285
2883.856796	187397.028456	55.275290
2883.467717	187156.355655	55.280295
2882.778935	186903.021899	55.285300
2882.311827	186662.631158	55.290305
2881.252795	186413.976877	55.295309
2880.712925	186155.801871	55.300314
2879.822413	185924.947276	55.305319
2879.164883	185682.327225	55.310324
2878.849843	185423.484601	55.315329
2877.677157	185173.633676	55.320333
2877.514337	184932.669417	55.325338
2876.800951	184692.709575	55.330343
2876.001017	184440.717259	55.335348
2875.326497	184193.604303	55.340353
2874.313445	183965.577741	55.345357
2873.995888	183712.469917	55.350362
2872.956895	183470.787088	55.355367
2872.356972	183226.097399	55.360372
2871.695449	182975.096324	55.365377
2871.062424	182745.883571	55.370381
2870.379065	182509.059999	55.375386
2869.908872	182269.023663	55.380391
2869.288276	182022.257587	55.385396
2868.817955	181780.532020	55.390401
2867.890030	181539.032888	55.395405
2867.378671	181283.183666	55.400410
2866.691550	181045.160051	55.405415
2866.001539	180809.631433	55.410420
2865.503113	180569.519777	55.415425
2864.642021	180325.816086	55.420429
2864.047325	180072.022428	55.425434
2863.078443	179834.622459	55.430439
2862.620923	179588.683817	55.435444
2862.044746	179346.581434	55.440449
2861.204950	179111.645445	55.445453
2860.772178	178870.477045	55.450458
2859.972863	178633.502051	55.455463
2859.219871	178383.737497	55.460468
2858.926033	178140.185308	55.465473
2857.981134	177896.788495	55.470477
2857.268450	177650.926840	55.475482
2856.446275	177408.899848	55.480487
2856.062222	177168.992630	55.485492
2855.612684	176920.473329	55.490497
2854.521457	176687.574815	55.495501
2854.045990	176446.821280	55.500506
2853.221564	176207.612549	55.505511
2852.897007	175972.803194	55.510516
2852.177695	175729.472261	55.515521
2851.290011	175480.191463	55.520525
2850.593786	175236.579952	55.525530
2849.887895	175005.728478	55.530535
2849.199520	174754.652573	55.535540
2848.543372	174518.441330	55.540545
2847.611543	174288.799795	55.545549
2847.416929	174046.311468	55.550554
2846.989652	173804.484636	55.555559
2846.095896	173559.426315	55.560564
2845.631349	173314.174321	55.565569
2844.781362	173078.485430	55.570573
2843.992315	172827.399201	55.575578
2843.294498	172594.474336	55.580583
2842.999312	172357.468143	55.585588
2842.100460	172108.832950	55.590593
2841.467067	171879.831899	55.595597
2840.989917	171624.074489	55.600602
2840.155760	171388.418469	55.605607
2839.796408	171141.458929	55.610612
2839.175654	170903.419222	55.615617
2838.397613	170654.010942	55.620621
2837.977548	170398.799259	55.625626
2836.949166	170161.744244	55.630631
2836.257121	169924.561094	55.635636
2835.599232	169672.202326	55.640641
2834.824942	169428.498560	55.645645
2834.363417	169184.428862	55.650650
2833.501931	168948.016076	55.655655
2832.898606	168697.498951	55.660660
2832.464727	168460.105808	55.665665
2831.590129	168215.840579	55.670669
2831.243977	167965.961462	55.675674
2830.035491	167739.606332	55.680679
2829.668792	167486.821492	55.685684
2829.266323	167236.536405	55.690689
2828.245805	167003.454315	55.695693
2827.504939	166750.174094	55.700698
2826.930212	166518.168843	55.705703
2826.340062	166274.862844	55.710708
2825.678945	166031.277182	55.715713
2824.659607	165785.740708	55.720717
2824.226045	165540.990460	55.725722
2823.471461	165302.866700	55.730727
2822.619788	165067.480987	55.735732
2822.537435	164821.446395	55.740737
2821.678445	164584.551729	55.745741
2821.019797	164342.947560	55.750746
2820.213222	164112.392608	55.755751
2819.421718	163851.447191	55.760756
2818.832138	163618.063594	55.765761
2818.042954	163380.097500	55.770765
2817.504719	163139.537480	55.775770
2817.038066	162909.673682	55.780775
2816.034684	162667.194182	55.785780
2815.733420	162426.308871	55.790785
2815.051157	162190.914666	55.795789
2814.474545	161945.486135	55.800794
2813.607128	161698.134568	55.805799
2813.147105	161457.624107	55.810804
2812.259200	161211.703126	55.815809
2811.700701	160979.831775	55.820813
2811.477081	160708.952620	55.825818
2810.373877	160430.573653	55.830823
2809.646543	160194.182472	55.835828
2809.336932	159937.613294	55.840833
2808.424983	159699.805239	55.845837
2807.709670	159450.893970	55.850842
2807.060649	159213.123809	55.855847
2806.634476	158971.175327	55.860852
2806.070028	158735.759697	55.865857
2805.077183	158484.407334	55.870861
2804.589060	158233.587065	55.875866
2803.616033	158000.135342	55.880871
2802.883461	157755.993495	55.885876
2802.314629	157520.319721	55.890881
2801.587293	157280.235823	55.895885
2801.051002	157035.610256	55.900890
2800.569741	156804.682058	55.905895
2799.878676	156554.414494	55.910900
2799.370726	156312.878711	55.915905
2798.020275	156079.016568	55.920909
2798.187473	155833.143940	55.925914
2797.250357	155595.164355	55.930919
2796.529917	155352.880788	55.935924
2795.905674	155099.740237	55.940929
2794.717492	154861.487706	55.945933
2794.213900	154626.624200	55.950938
2793.680838	154397.970377	55.955943
2793.204597	154150.038013	55.960948
2792.493183	153916.814009	55.965953
2791.355087	153671.430620	55.970957
2790.988672	153427.922497	55.975962
2790.481338	153196.870227	55.980967
2789.481293	152962.948550	55.985972
2789.063304	152723.851809	55.990977
2788.258328	152491.249915	55.995981
2787.438844	152248.495787	56.000986
2786.842670	152009.635746	56.005991
2785.971176	151782.044742	56.010996
2785.541535	151548.652735	56.016001
2784.765312	151317.274713	56.021005
2784.498357	151078.153134	56.026010
2783.498328	150839.251079	56.031015
2782.566715	150615.185715	56.036020
2782.464477	150376.081259	56.041025
2781.439336	150149.415545	56.046029
2780.955156	149903.524188	56.051034
2780.093120	149681.843680	56.056039
2779.754254	149443.304611	56.061044
2779.217085	149209.018382	56.066049
2778.041883	148969.649294	56.071053
2777.624946	148731.559933	56.076058
2776.976962	148505.748282	56.081063
2776.006726	148277.269407	56.086068
2775.533495	148036.258167	56.091073
2774.990673	147811.832741	56.096077
2774.305045	147574.391795	56.101082
2773.630519	147345.974352	56.106087
2772.666775	147107.703973	56.111092
2772.182392	146874.163432	56.116097
2771.123542	146648.302799	56.121101
2770.853812	146415.977077	56.126106
2770.263369	146193.794564	56.131111
2769.315250	145962.774222	56.136116
2768.820014	145730.578184	56.141121
2767.908690	145506.214607	56.146125
2767.322130	145277.543884	56.151130
2766.906140	145057.629202	56.156135
2766.447966	144817.821750	56.161140
2766.153208	144586.263190	56.166145
2765.179293	144360.354590	56.171149
2764.284762	144107.443511	56.176154
2763.375317	143882.811639	56.181159
2762.931582	143657.700967	56.186164
2762.302253	143422.671271	56.191169
2761.706425	143195.491276	56.196173
2761.357880	142962.275875	56.201178
2760.228685	142725.322861	56.206183
2759.424242	142497.291513	56.211188
2758.853363	142264.472386	56.216193
2758.083481	142045.842167	56.221197
2757.522004	141812.021112	56.226202
2756.991883	141588.667302	56.231207
2756.342509	141344.367880	56.236212
2755.833676	141121.535076	56.241217
2755.065613	140891.362451	56.246221
2754.403052	140656.981718	56.251226
2753.456887	140437.704748	56.256231
2753.097186	140200.649335	56.261236
2752.673177	139968.408889	56.266241
2751.644940	139744.969592	56.271245
2751.233284	139507.254406	56.276250
2750.435910	139276.806420	56.281255
2749.591828	139043.419853	56.286260
2749.352398	138818.223418	56.291265
2748.474652	138584.820330	56.296269
2747.960770	138350.167102	56.301274
2746.866385	138116.128590	56.306279
2746.350596	137893.828879	56.311284
2745.877570	137657.777029	56.316289
2745.037227	137436.421501	56.321293
2744.577982	137195.250981	56.326298
2743.683614	136965.039437	56.331303
2743.285372	136741.078080	56.336308
2742.532808	136500.162952	56.341313
2741.843314	136280.253200	56.346317
2741.324521	136043.014514	56.351322
2740.374929	135810.203589	56.356327
2739.659182	135585.361174	56.361332
2738.944326	135351.614694	56.366337
2738.184780	135138.965969	56.371341
2737.815841	134903.402399	56.376346
2737.465241	134669.667184	56.381351
2736.616114	134445.972598	56.386356
2735.847586	134204.748553	56.391361
2735.172046	133982.033629	56.396365
2734.714085	133736.470459	56.401370
2733.930130	133517.384072	56.406375
2733.237453	133287.893584	56.411380
2732.675531	133053.074271	56.416385
2731.840776	132831.600232	56.421389
2731.170916	132597.170126	56.426394
2730.384105	132376.149308	56.431399
2729.633557	132132.322935	56.436404
2728.910292	131914.572932	56.441409
2728.021834	131688.835420	56.446413
2727.845812	131457.753406	56.451418
2727.015699	131236.862579	56.456423
2726.279146	131015.336235	56.461428
2725.911036	130785.522231	56.466433
2725.234536	130555.543007	56.471437
2724.465304	130322.442952	56.476442
2723.642452	130100.670688	56.481447
2723.105789	129862.939501	56.486452
2722.358801	129637.106999	56.491457
2721.433275	129424.780963	56.496461
2721.248265	129192.855157	56.501466
2720.529828	128971.659519	56.506471
2719.720665	128743.049759	56.511476
2719.197035	128517.101983	56.516481
2718.606451	128296.856719	56.521485
2717.987380	128059.306299	56.526490
2717.188688	127839.427845	56.531495
2716.390115	127606.151820	56.536500
2716.071417	127379.012349	56.541505
2715.024042	127152.968120	56.546509
2714.541544	126923.318230	56.551514
2713.898360	126702.814546	56.556519
2712.918276	126473.107529	56.561524
2712.468881	126241.819742	56.566529
2711.756448	126030.514604	56.571533
2711.219383	125798.533238	56.576538
2710.246250	125592.975037	56.581543
2709.747865	125357.829022	56.586548
2709.200531	125116.228688	56.591553
2708.232256	124905.226768	56.596557
2707.580631	124685.604222	56.601562
2707.261997	124459.047678	56.606567
2706.409327	124237.936686	56.611572
2706.333252	124012.970935	56.616577
2704.964163	123785.748297	56.621581
2704.306630	123552.433675	56.626586
2703.273169	123341.378067	56.631591
2702.706681	123119.405470	56.636596
2702.340375	122900.234769	56.641601
2701.645481	122683.873478	56.646605
2701.438484	122455.741453	56.651610
2700.493311	122238.813885	56.656615
2699.836958	122012.572676	56.661620
2699.429875	121790.331867	56.666625
2698.674517	121570.509901	56.671629
2698.039301	121339.344259	56.676634
2697.142313	121123.141912	56.681639
2696.487654	120895.627456	56.686644
2695.931441	120663.185424	56.691649
2694.878504	120444.600797	56.696653
2694.194234	120226.073845	56.701658
2693.902858	120006.788111	56.706663
2693.220055	119788.569285	56.711668
2692.568418	119565.332027	56.716673
2691.721881	119347.701467	56.721677
2691.246152	119122.459395	56.726682
2690.566917	118903.269711	56.731687
2690.107077	118678.524109	56.736692
2689.584344	118452.717556	56.741697
2688.821303	118231.420135	56.746701
2688.162745	118002.337960	56.751706
2687.671319	117786.422571	56.756711
2686.588717	117558.116128	56.761716
2685.806431	117326.336228	56.766721
2685.338813	117108.372328	56.771725
2684.667470	116874.134966	56.776730
2683.870107	116659.553357	56.781735
2683.308246	116448.370341	56.786740
2683.035862	116211.073318	56.791745
2682.148445	115995.673619	56.796749
2681.419474	115765.657590	56.801754
2681.095961	115546.014675	56.806759
2680.177566	115319.009647	56.811764
2679.502781	115089.410041	56.816769
2678.491669	114870.034212	56.821773
2678.178870	114646.138275	56.826778
2677.135559	114422.042687	56.831783
2676.667266	114198.238800	56.836788
2675.918396	113975.763457	56.841793
2675.157172	113763.828136	56.846797
2674.615744	113537.502848	56.851802
2673.679765	113326.519195	56.856807
2673.142116	113095.741710	56.861812
2672.509058	112872.254923	56.866817
2671.867744	112657.504594	56.871821
2671.410456	112432.178690	56.876826
2670.542079	112221.447460	56.881831
2669.808898	112000.453148	56.886836
2669.163293	111771.450251	56.891841
2668.544790	111556.172634	56.896845
2667.867575	111339.186289	56.901850
2666.958408	111130.482544	56.906855
2666.440616	110912.490966	56.911860
2665.810144	110683.889135	56.916865
2665.010308	110477.045706	56.921869
2664.911141	110256.328145	56.926874
2664.138998	110035.871485	56.931879
2663.340842	109814.538811	56.936884
2663.000739	109593.059393	56.941889
2662.137778	109376.113313	56.946893
2661.467538	109154.918594	56.951898
2660.739720	108929.045423	56.956903
2660.270034	108704.326432	56.961908
2659.758233	108480.460153	56.966913
2658.443194	108266.013228	56.971917
2658.004491	108043.478297	56.976922
2657.676168	107824.329112	56.981927
2656.670347	107608.576204	56.986932
2656.252228	107387.604983	56.991937
2655.465064	107166.078741	56.996941
2654.604019	106941.913887	57.001946
2653.671505	106725.941459	57.006951
2652.931916	106510.428969	57.011956
2652.475633	106295.051172	57.016961
2651.764283	106087.761277	57.021965
2651.375631	105874.432323	57.026970
2650.510343	105653.598535	57.031975
2650.026344	105448.124505	57.036980
2649.290685	105215.992933	57.041985
2648.656783	105002.824773	57.046989
2648.145645	104786.860058	57.051994
2647.203941	104572.304243	57.056999
2646.505511	104364.380013	57.062004
2645.504740	104139.870028	57.067009
2645.143813	103928.641350	57.072013
2644.792028	103722.450597	57.077018
2643.976739	103513.448369	57.082023
2643.378222	103292.042154	57.087028
2642.621213	103074.704428	57.092033
2642.074765	102860.666052	57.097037
2641.478620	102645.755645	57.102042
2640.807794	102435.096895	57.107047
2640.192671	102218.106171	57.112052
2639.664795	101992.945236	57.117057
2638.431112	101785.896048	57.122061
2638.329949	101556.319731	57.127066
2637.556962	101341.214518	57.132071
2637.018462	101120.840516	57.137076
2635.978589	100902.831767	57.142081
2635.144958	100685.839070	57.147085
2634.693493	100475.251945	57.152090
2633.937613	100263.852237	57.157095
2633.061952	100043.839962	57.162100
2632.898165	99838.662042	57.167105
2631.895811	99631.849013	57.172109
2631.332924	99413.220398	57.177114
2630.941341	99201.315905	57.182119
2630.093092	98978.835513	57.187124
2629.417451	98766.770683	57.192129
2628.862848	98550.089899	57.197133
2628.169295	98332.443659	57.202138
2627.417828	98121.982519	57.207143
2626.668773	97908.503707	57.212148
2626.275231	97688.266176	57.217153
2625.062692	97477.097492	57.222157
2624.777941	97260.728596	57.227162
2624.021634	97054.489562	57.232167
2623.098775	96845.684660	57.237172
2622.943039	96627.087746	57.242177
2621.784753	96420.632718	57.247181
2621.743725	96205.110452	57.252186
2620.671815	95997.465883	57.257191
2619.975896	95792.928437	57.262196
2619.478208	95574.433863	57.267201
2618.815725	95362.049655	57.272205
2618.034538	95148.252928	57.277210
2617.361026	94934.339686	57.282215
2616.746675	94720.799613	57.287220
2616.228283	94512.300877	57.292225
2615.527041	94296.362310	57.297229
2615.014596	94085.786441	57.302234
2613.944194	93875.954162	57.307239
2613.715398	93662.978168	57.312244
2613.018170	93446.647598	57.317249
2611.980590	93244.387942	57.322253
2611.722364	93019.367380	57.327258
2610.913553	92816.035335	57.332263
2610.105453	92600.307590	57.337268
2609.591429	92378.320819	57.342273
2608.572222	92166.524306	57.347277
2608.223849	91955.378107	57.352282
2607.563459	91753.148295	57.357287
2606.757048	91540.563087	57.362292
2606.441037	91325.080441	57.367297
2605.082434	91107.089221	57.372301
2604.987143	90905.221461	57.377306
2604.263303	90689.023364	57.382311
2603.673227	90484.764922	57.387316
2603.183637	90271.120842	57.392321
2602.415541	90057.174233	57.397325
2601.760663	89832.172764	57.402330
2600.917533	89624.944275	57.407335
2600.132514	89413.377983	57.412340
2599.835004	89200.106986	57.417345
2598.930788	88990.427753	57.422349
2598.147367	88775.202645	57.427354
2597.539516	88558.284353	57.432359
2596.860352	88360.057681	57.437364
2596.226161	88146.558676	57.442369
2595.702212	87934.686368	57.447373
2595.293119	87717.446968	57.452378
2594.369025	87497.038972	57.457383
2593.313457	87287.057773	57.462388
2593.071386	87073.519854	57.467393
2592.166605	86866.669719	57.472397
2591.492416	86653.407301	57.477402
2590.928018	86452.517209	57.482407
2590.408585	86241.396148	57.487412
2589.872807	86025.468067	57.492417
2589.017655	85821.491887	57.497421
2588.426664	85603.022004	57.502426
2587.622869	85396.131954	57.507431
2587.052369	85176.832714	57.512436
2586.228439	84967.743933	57.517441
2585.366297	84763.075281	57.522445
2584.904138	84552.684419	57.527450
2584.340130	84348.111956	57.532455
2583.855625	84137.608286	57.537460
2582.871097	83925.854776	57.542465
2581.984855	83723.133286	57.547469
2581.688245	83505.449572	57.552474
2580.994720	83295.158514	57.557479
2580.290683	83085.701568	57.562484
2579.710326	82873.850132	57.567489
2578.927254	82670.266654	57.572493
2578.313623	82466.683638	57.577498
2577.612282	82249.393903	57.582503
2577.094948	82038.973325	57.587508
2576.371484	81825.012746	57.592513
2575.512896	81632.067828	57.597517
2575.070007	81412.685858	57.602522
2574.276366	81215.101312	57.607527
2573.437085	81011.802645	57.612532
2573.145485	80800.414337	57.617537
2572.454727	80594.827200	57.622541
2571.789936	80376.327851	57.627546
2570.949916	80167.257433	57.632551
2570.132299	79954.452668	57.637556
2569.774101	79750.240787	57.642561
2568.799665	79549.183279	57.647565
2568.617941	79333.666671	57.652570
2568.011150	79125.476019	57.657575
2567.118155	78917.440553	57.662580
2566.417015	78706.252481	57.667585
2565.434877	78501.809558	57.672589
2565.023315	78284.736964	57.677594
2564.489163	78088.573185	57.682599
2563.687137	77878.645299	57.687604
2563.081688	77670.982385	57.692609
2561.964965	77464.144017	57.697613
2561.220534	77256.944558	57.702618
2560.681887	77052.521773	57.707623
2560.045413	76862.323479	57.712628
2559.814187	76652.640826	57.717633
2558.803112	76456.270393	57.722637
2558.331923	76241.510006	57.727642
2557.599019	76043.306213	57.732647
2556.984247	75841.644947	57.737652
2556.093920	75635.365795	57.742657
2555.344361	75438.513829	57.747661
2554.942368	75225.254880	57.752666
2554.526024	75024.305264	57.757671
2553.468406	74819.892052	57.762676
2553.022773	74619.293238	57.767681
2552.417861	74414.685641	57.772685
2551.796284	74201.991802	57.777690
2551.150650	74008.140468	57.782695
2550.615099	73802.254571	57.787700
2549.983841	73598.584436	57.792705
2549.043217	73396.257866	57.797709
2548.554213	73186.544147	57.802714
2547.956650	72988.456496	57.807719
2547.200718	72776.185465	57.812724
2547.033062	72569.632992	57.817729
2546.134076	72357.724839	57.822733
2545.411868	72129.604334	57.827738
2544.618727	71922.156705	57.832743
2543.830010	71720.595858	57.837748
2543.427433	71518.361343	57.842753
2542.682426	71317.893601	57.847757
2541.826294	71102.127633	57.852762
2541.219696	70888.852062	57.857767
2540.617121	70689.616041	57.862772
2539.811773	70476.813496	57.867777
2538.932339	70271.227485	57.872781
2538.550162	70063.905128	57.877786
2537.926124	69864.503432	57.882791
2537.166737	69659.462186	57.887796
2536.534887	69447.378006	57.892801
2535.537979	69258.797335	57.897805
2535.248308	69049.716344	57.902810
2534.534987	68842.839348	57.907815
2533.539052	68643.375925	57.912820
2533.000471	68434.676631	57.917825
2532.306711	68242.212875	57.922829
2531.951927	68032.424612	57.927834
2531.180078	67831.863483	57.932839
2530.444666	67634.598551	57.937844
2530.202122	67422.069162	57.942849
2529.445299	67225.806147	57.947853
2528.528495	67018.473970	57.952858
2527.809141	66813.886795	57.957863
2527.212931	66612.043647	57.962868
2526.501432	66404.375125	57.967873
2525.812125	66207.117329	57.972877
2525.297844	66002.544183	57.977882
2524.584993	65801.975596	57.982887
2523.747585	65597.679602	57.987892
2523.735832	65388.334087	57.992897
2522.473764	65187.843084	57.997901
2521.819873	64984.132453	58.002906
2520.949057	64786.461929	58.007911
2520.441092	64583.049046	58.012916
2519.731364	64380.313066	58.017921
2519.157041	64189.403049	58.022925
2518.675617	63980.381566	58.027930
2518.205072	63781.923330	58.032935
2517.329250	63576.787287	58.037940
2517.100503	63362.910287	58.042945
2515.937511	63161.465350	58.047949
2515.495063	62961.963148	58.052954
2514.878910	62758.371455	58.057959
2514.369275	62556.278431	58.062964
2513.603104	62345.420288	58.067969
2512.345912	62145.257927	58.072973
2511.967673	61930.249244	58.077978
2511.306467	61732.690994	58.082983
2510.293299	61540.787911	58.087988
2509.823490	61336.871630	58.092993
2509.316074	61137.743919	58.097997
2508.666950	60927.566779	58.103002
2507.914790	60728.241567	58.108007
2507.309201	60532.608633	58.113012
2506.621547	60328.633276	58.118017
2505.641610	60129.834839	58.123021
2505.313204	59922.998972	58.128026
2504.325532	59727.134223	58.133031
2503.534223	59538.122336	58.138036
2503.223054	59333.480790	58.143041
2502.461652	59143.186093	58.148045
2501.598475	58936.689590	58.153050
2500.840760	58749.000324	58.158055
2500.539882	58555.191435	58.163060
2499.901904	58357.133082	58.168065
2498.962369	58168.266128	58.173069
2498.761405	57965.195230	58.178074
2497.975268	57769.037295	58.183079
2497.151004	57574.691655	58.188084
2496.629003	57369.462468	58.193089
2495.784889	57175.026026	58.198093
2495.147876	56976.178239	58.203098
2494.394388	56785.925310	58.208103
2493.993853	56584.059543	58.213108
2493.371730	56382.791311	58.218113
2492.396470	56199.090039	58.223117
2491.939580	55996.480008	58.228122
2491.512101	55798.985234	58.233127
2490.602674	55598.562315	58.238132
2490.125209	55400.101777	58.243137
2489.400161	55208.309784	58.248141
2489.041812	54999.776834	58.253146
2487.882800	54801.541554	58.258151
2487.160961	54599.881333	58.263156
2486.707952	54398.345276	58.268161
2485.915194	54209.207467	58.273165
2485.336520	54009.455155	58.278170
2484.617332	53812.607077	58.283175
2483.938330	53619.637661	58.288180
2483.666672	53423.140551	58.293185
2482.577393	53225.588482	58.298189
2482.169610	53022.835743	58.303194
2481.502503	52836.388338	58.308199
2480.668013	52637.606100	58.313204
2480.095461	52434.281633	58.318209
2479.502204	52239.699409	58.323213
2478.699304	52035.200823	58.328218
2478.000050	51842.168014	58.333223
2477.177782	51650.685077	58.338228
2476.980237	51455.096108	58.343233
2476.311527	51262.953764	58.348237
2475.536924	51055.854489	58.353242
2474.751121	50861.959903	58.358247
2474.083773	50656.458724	58.363252
2473.812776	50459.636046	58.368257
2472.957167	50268.423005	58.373261
2472.506537	50060.239693	58.378266
2471.933153	49856.988629	58.383271
2470.932607	49654.674482	58.388276
2470.256413	49450.039565	58.393281
2469.353793	49257.171075	58.398285
2469.070877	49062.713123	58.403290
2468.254320	48863.937970	58.408295
2467.517861	48668.913961	58.413300
2466.914549	48458.872068	58.418305
2466.313853	48273.160484	58.423309
2465.827312	48070.399970	58.428314
2464.991197	47867.975574	58.433319
2464.312311	47674.392729	58.438324
2463.716525	47473.092572	58.443329
2462.810648	47273.925403	58.448333
2462.361595	47074.738662	58.453338
2461.681397	46875.625597	58.458343
2461.233016	46683.601862	58.463348
2460.923395	46474.957183	58.468353
2459.428946	46279.355158	58.473357
2458.768824	46079.396949	58.478362
2458.194334	45883.596524	58.483367
2457.597928	45693.976241	58.488372
2456.845422	45482.516040	58.493377
2456.369697	45288.582299	58.498381
2455.545633	45093.152858	58.503386
2454.686083	44909.383791	58.508391
2454.255441	44718.188372	58.513396
2453.701327	44512.297389	58.518401
2453.082711	44309.850812	58.523405
2452.324623	44117.584692	58.528410
2451.736479	43926.182501	58.533415
2450.859580	43721.601312	58.538420
2450.233050	43519.857786	58.543425
2449.379148	43337.021531	58.548429
2448.896903	43127.877829	58.553434
2448.160218	42935.912294	58.558439
2447.200183	42754.253355	58.563444
2446.520424	42560.907187	58.568449
2445.647576	42368.479300	58.573453
2445.119954	42183.487682	58.578458
2444.660002	41992.766352	58.583463
2444.024779	41796.708214	58.588468
2443.358936	41615.621743	58.593473
2442.516128	41424.227363	58.598477
2442.114271	41237.897698	58.603482
2441.784182	41050.309544	58.608487
2440.754068	40859.264189	58.613492
2440.468358	40657.240594	58.618497
2439.359706	40475.847321	58.623501
2438.991549	40281.215499	58.628506
2438.273603	40090.499153	58.633511
2437.431975	39900.519170	58.638516
2436.943855	39705.394298	58.643521
2436.149042	39518.032486	58.648525
2435.583300	39318.595485	58.653530
2435.059090	39134.170412	58.658535
2434.210427	38946.088234	58.663540
2433.712034	38747.067749	58.668545
2432.783280	38561.565219	58.673549
2432.288806	38359.759859	58.678554
2431.594599	38180.280769	58.683559
2431.082820	37987.735547	58.688564
2430.313373	37787.145669	58.693569
2429.487145	37607.233518	58.698573
2428.970882	37404.529199	58.703578
2428.186736	37224.974850	58.708583
2427.423115	37033.812979	58.713588
2426.596430	36838.915248	58.718593
2425.888231	36658.694091	58.723597
2425.238395	36464.208921	58.728602
2424.948572	36285.461880	58.733607
2424.205339	36096.751147	58.738612
2423.267951	35908.111243	58.743617
2422.731015	35732.379340	58.748621
2422.073329	35542.276577	58.753626
2421.493005	35349.968193	58.758631
2420.598485	35171.821979	58.763636
2420.184666	34976.102623	58.768641
2419.581255	34796.167671	58.773645
2419.024695	34609.979248	58.778650
2418.032816	34427.299600	58.783655
2417.248281	34235.256044	58.788660
2417.101373	34045.501742	58.793665
2416.174253	33862.132046	58.798669
2415.630124	33674.730320	58.803674
2414.952469	33490.443241	58.808679
2414.124946	33313.922958	58.813684
2413.591667	33118.267949	58.818689
2412.654760	32944.114270	58.823693
2412.059474	32751.932901	58.828698
2411.058543	32577.406015	58.833703
2410.514363	32389.494053	58.838708
2410.386264	32201.425001	58.843713
2409.365624	32025.363048	58.848717
2409.088904	31840.665601	58.853722
2408.443148	31650.208537	58.858727
2407.446171	31477.908139	58.863732
2406.897011	31280.605355	58.868737
2406.198319	31096.228050	58.873741
2405.656296	30912.627547	58.878746
2404.492027	30739.353195	58.883751
2403.881087	30543.941533	58.888756
2403.322592	30360.182287	58.893761
2402.272530	30197.378309	58.898765
2401.707172	30013.977965	58.903770
2401.197419	29834.298326	58.908775
2400.553710	29664.059243	58.913780
2400.214623	29484.048251	58.918785
2399.589061	29309.572201	58.923789
2398.603853	29124.581390	58.928794
2397.812608	28945.428542	58.933799
2397.159248	28770.994231	58.938804
2396.628509	28585.447645	58.943809
2395.869950	28417.737677	58.948813
2395.421263	28241.707642	58.953818
2394.493738	28061.734485	58.958823
2393.902483	27889.361554	58.963828
2393.372075	27705.223143	58.968833
2392.685589	27531.385567	58.973837
2391.749004	27355.120165	58.978842
2391.554868	27175.433893	58.983847
2390.738966	27003.557795	58.988852
2390.280213	26828.364557	58.993857
2389.407470	26650.270405	58.998861
2388.889746	26468.937069	59.003866
2388.307425	26301.295208	59.008871
2387.388861	26120.398997	59.013876
2386.839822	25935.011903	59.018881
2385.932812	25766.782532	59.023885
2385.612278	25581.356939	59.028890
2384.886665	25410.333305	59.033895
2384.537887	25231.268108	59.038900
2383.880619	25041.516174	59.043905
2382.966370	24869.843406	59.048909
2382.291885	24687.344919	59.053914
2381.573059	24508.584161	59.058919
2380.561085	24326.064308	59.063924
2380.228573	24150.018433	59.068929
2379.437468	23979.647467	59.073933
2378.817736	23790.866276	59.078938
2378.262194	23629.221711	59.083943
2377.330523	23446.320843	59.088948
2377.175470	23272.176329	59.093953
2376.273624	23093.728870	59.098957
2375.610385	22911.214847	59.103962
2375.080339	22737.978242	59.108967
2374.369502	22552.838233	59.113972
2373.784749	22381.462860	59.118977
2372.802071	22209.940005	59.123981
2372.252884	22024.264839	59.128986
2371.654743	21846.808168	59.133991
2370.545301	21668.244543	59.138996
2370.246498	21497.716175	59.144001
2369.334242	21323.187898	59.149005
2368.620698	21149.117233	59.154010
2368.276532	20971.948282	59.159015
2367.577296	20804.475631	59.164020
2367.111582	20614.860378	59.169025
2366.350647	20446.659069	59.174029
2365.638639	20270.917553	59.179034
2364.865677	20099.595871	59.184039
2364.117102	19930.905395	59.189044
2363.690994	19751.029620	59.194049
2363.057763	19572.163837	59.199053
2362.304363	19398.239571	59.204058
2361.717458	19224.571109	59.209063
2360.986159	19047.325250	59.214068
2360.183903	18872.070776	59.219073
2359.255715	18707.358027	59.224077
2358.527603	18532.845219	59.229082
2358.134189	18358.116666	59.234087
2357.271961	18194.615841	59.239092
2357.061207	18017.623933	59.244097
2356.442366	17855.328316	59.249101
2355.723227	17677.926662	59.254106
2354.859473	17511.742350	59.259111
2353.942063	17338.301920	59.264116
2353.257255	17158.527270	59.269121
2352.581639	17004.401548	59.274125
2352.239621	16824.694403	59.279130
2351.369130	16661.848775	59.284135
2350.555406	16491.511973	59.289140
2350.201189	16315.224806	59.294145
2349.128405	16153.031912	59.299149
2348.245927	15994.566360	59.304154
2347.703892	15825.884798	59.309159
2346.794544	15670.461916	59.314164
2346.575163	15503.441249	59.319169
2345.665876	15354.220463	59.324173
2345.219127	15186.896099	59.329178
2344.624706	15025.384860	59.334183
2343.853880	14857.325538	59.339188
2343.345417	14689.311484	59.344193
2342.579679	14534.911221	59.349197
2342.147789	14370.215183	59.354202
2341.439435	14206.758829	59.359207
2340.529193	14042.090259	59.364212
2340.370599	13865.892591	59.369217
2339.323211	13707.435789	59.374221
2338.812788	13544.308069	59.379226
2338.137405	13382.426723	59.384231
2337.232981	13220.913896	59.389236
2336.758630	13061.553558	59.394241
2335.840852	12898.310178	59.399245
2335.644140	12728.384919	59.404250
2334.192417	12571.569451	59.409255
2334.002374	12404.735143	59.414260
2333.031237	12236.964488	59.419265
2332.346302	12082.070266	59.424269
2331.628435	11928.098290	59.429274
2331.265835	11766.501259	59.434279
2330.222829	11607.806830	59.439284
2329.923597	11448.799207	59.444289
2329.149708	11293.069426	59.449293
2328.532873	11140.530424	59.454298
2327.775077	10986.179233	59.459303
2326.961427	10836.710212	59.464308
2326.805571	10676.502867	59.469313
2325.991887	10514.537114	59.474317
2325.197806	10353.020348	59.479322
2324.517487	10194.972988	59.484327
2324.046177	10044.278003	59.489332
2323.075407	9879.845361	59.494337
2322.196480	9733.883012	59.499341
2321.542238	9572.144669	59.504346
2320.970491	9426.707830	59.509351
2320.391045	9271.590493	59.514356
2319.956094	9105.393956	59.519361
2319.215914	8962.742355	59.524365
2318.588219	8815.438879	59.529370
2317.938344	8657.164275	59.534375
2316.942567	8508.718562	59.539380
2316.400970	8353.428119	59.544385
2315.822008	8204.520469	59.549389
2315.013299	8053.344200	59.554394
2314.279071	7897.953698	59.559399
2313.238142	7752.037400	59.564404
2313.051132	7586.330708	59.569409
2311.919454	7446.071099	59.574413
2311.145389	7298.326410	59.579418
2310.706147	7158.153353	59.584423
2310.213702	7011.945043	59.589428
2309.258561	6851.004308	59.594433
2308.438969	6717.012821	59.599437
2307.992718	6579.313942	59.604442
2307.436223	6434.732723	59.609447
2306.737730	6294.337495	59.614452
2306.249219	6151.613118	59.619457
2305.200699	6009.770144	59.624461
2304.383574	5865.804926	59.629466
2303.910748	5721.306482	59.634471
2303.215986	5586.592228	59.639476
2302.788817	5436.966627	59.644481
2301.952557	5308.834820	59.649485
2301.318301	5174.128111	59.654490
2300.726198	5038.971840	59.659495
2299.442040	4908.287811	59.664500
2299.319743	4757.589730	59.669505
2298.588043	4621.122405	59.674509
2297.710331	4496.825029	59.679514
2297.220825	4360.692409	59.684519
2296.480034	4226.090071	59.689524
2295.486091	4093.972663	59.694529
2294.459729	3981.476901	59.699533
2293.756882	3851.563415	59.704538
2293.005592	3735.413469	59.709543
2291.805744	3620.873599	59.714548
2290.973654	3497.209152	59.719553
2290.177254	3400.463650	59.724557
2289.149215	3299.991796	59.729562
2288.438913	3203.391673	59.734567
2287.589872	3101.678174	59.739572
2287.072695	2996.864438	59.744577
2286.247168	2918.548255	59.749581
2285.533736	2817.927259	59.754586
2284.899484	2737.964107	59.759591
2284.174328	2649.468141	59.764596
2283.439093	2556.160261	59.769601
2282.325594	2483.556302	59.774605
2281.860718	2391.185322	59.779610
2281.177936	2301.286433	59.784615
2280.420176	2238.996522	59.789620
2279.893717	2156.451580	59.794625
2278.798830	2090.219690	59.799629
2278.327740	2007.910491	59.804634
2277.830832	1932.706735	59.809639
2276.658608	1865.035461	59.814644
2276.179039	1791.190862	59.819649
2275.576487	1730.433671	59.824653
2274.758547	1654.543320	59.829658
2274.118913	1583.441959	59.834663
2273.142789	1521.258345	59.839668
2272.972884	1457.822557	59.844673
2271.589101	1401.923892	59.849677
2270.777521	1340.913632	59.854682
2270.478239	1285.825206	59.859687
2269.328105	1243.155963	59.864692
2268.935029	1185.812412	59.869697
2268.087712	1139.430044	59.874701
2266.864929	1088.857658	59.879706
2266.215472	1047.761671	59.884711
2265.559204	1015.107921	59.889716
2264.925524	976.480279	59.894721
2264.080810	946.274377	59.899725
2263.319145	889.419446	59.904730
2262.522901	849.183988	59.909735
2261.645460	826.534171	59.914740
2261.329308	792.017187	59.919745
2260.574609	755.384710	59.924750
2259.650080	726.268331	59.929754
2259.292560	706.107765	59.934759
2258.894720	693.687130	59.939764
2258.424800	646.748094	59.944769
2257.183550	618.008638	59.949774
2257.007947	573.911669	59.954778
2256.262300	558.748496	59.959783
2255.441644	526.064356	59.964788
2255.035152	496.014621	59.969793
2254.058525	476.221479	59.974798
2253.480445	444.437429	59.979802
2252.815433	413.197937	59.984807
2251.985642	395.639247	59.989812
2251.519213	377.965376	59.994817
2250.598484	360.753924	59.999822
2250.161202	335.328747	60.004826
2249.096550	318.413014	60.009831
2248.049901	292.430865	60.014836
2247.638827	277.516932	60.019841
2246.453549	262.017708	60.024846
2245.906839	251.159524	60.029850
2245.333731	245.782775	60.034855
2244.991066	236.431478	60.039860
2244.800019	212.624192	60.044865
2243.799259	205.023786	60.049870
2243.215036	187.631421	60.054874
2242.510224	165.306162	60.059879
2241.480486	157.077970	60.064884
2241.111688	135.874382	60.069889
2240.701628	144.556718	60.074894
2240.086677	118.514292	60.079898
2239.139733	108.498783	60.084903
2238.418182	100.895149	60.089908
2238.098556	78.627205	60.094913
2237.126260	78.802062	60.099918
2235.924656	63.693607	60.104922
2235.144388	49.691673	60.109927
2234.530389	47.972407	60.114932
2234.247249	40.721916	60.119937
2232.987594	40.182211	60.124942
2232.625850	41.584957	60.129946
2232.292040	34.550680	60.134951
2231.175390	38.883514	60.139956
2230.885565	36.751678	60.144961
2230.348658	46.269424	60.149966
2229.281488	37.153045	60.154970
2228.564255	36.886869	60.159975
2228.129420	46.134515	60.164980
2227.641997	37.796713	60.169985
2226.320352	52.198544	60.174990
2226.468768	46.855662	60.179994
2225.581394	47.745659	60.184999
2224.872744	46.423062	60.190004
2223.857950	43.349593	60.195009
2223.306829	48.715595	60.200014
2223.090217	46.117947	60.205018
2222.195755	45.854654	60.210023
2221.502001	60.265708	60.215028
2221.500283	42.686494	60.220033
2220.710992	51.883132	60.225038
2219.725713	45.546755	60.230042
2219.146539	43.241608	60.235047
2217.986594	47.436227	60.240052
2217.858279	44.092813	60.245057
2217.433821	45.194826	60.250062
2216.588498	45.199727	60.255066
2216.184881	47.358226	60.260071
2214.957353	56.728476	60.265076
2214.150234	55.968745	60.270081
2213.483870	59.681339	60.275086
2213.257313	60.252028	60.280090
2212.666331	54.542279	60.285095
2211.684668	41.553250	60.290100
2211.597365	45.727530	60.295105
2210.978403	63.596277	60.300110
2210.534024	56.010213	60.305114
2209.846209	48.327142	60.310119
2208.107339	62.035030	60.315124
2207.955263	45.766559	60.320129
2207.149345	56.421476	60.325134
2206.318322	58.062688	60.330138
2205.969067	59.463457	60.335143
2205.529532	57.737022	60.340148
2205.023999	51.226763	60.345153
2204.109305	51.666905	60.350158
2203.364208	46.117239	60.355162
2202.794819	51.669083	60.360167
2202.016699	55.383637	60.365172
2201.403437	47.736055	60.370177
2200.551681	56.370133	60.375182
2200.648148	57.548793	60.380186
2200.275074	46.748392	60.385191
2198.839048	50.363876	60.390196
2197.875809	47.242812	60.395201
2197.553229	53.428911	60.400206
2197.165159	49.049567	60.405210
2196.740713	52.733246	60.410215
2195.577629	57.554472	60.415220
2195.012893	47.945202	60.420225
2194.294462	47.862165	60.425230
2193.165335	47.689731	60.430234
2192.964769	49.707202	60.435239
2191.860145	53.202300	60.440244
2191.792017	49.045033	60.445249
2191.315233	51.746615	60.450254
2190.805130	45.334866	60.455258
2190.059233	42.354380	60.460263
2188.882425	56.129232	60.465268
2188.503408	45.596304	60.470273
2187.987668	58.405202	60.475278
2187.269220	51.498185	60.480282
2186.471743	48.904379	60.485287
2185.560836	55.070268	60.490292
2185.175878	51.669793	60.495297
2184.283976	54.773151	60.500302
2183.752749	50.919606	60.505306
2183.406797	49.905359	60.510311
2182.549801	57.224997	60.515316
2182.225188	47.093476	60.520321
2181.065263	55.456304	60.525326
2180.456621	52.233254	60.530330
2179.592172	49.541257	60.535335
2178.612144	60.129181	60.540340
2178.403076	48.709786	60.545345
2178.160668	60.831878	60.550350
2177.862532	52.629643	60.555354
2176.692307	47.166358	60.560359
2175.802254	56.328528	60.565364
2174.985609	49.623191	60.570369
2174.456911	57.042144	60.575374
2174.496043	60.381023	60.580378
2173.542031	51.674097	60.585383
2172.137425	62.020279	60.590388
2172.548275	55.419836	60.595393
2171.056584	57.214765	60.600398
2170.797221	61.170324	60.605402
2170.480541	52.860637	60.610407
2169.030588	62.330856	60.615412
2168.606826	52.552558	60.620417
2168.594628	56.505175	60.625422
2167.504512	62.757856	60.630426
2166.270331	60.230186	60.635431
2165.845400	66.662783	60.640436
2165.952242	60.241467	60.645441
2165.050262	59.971501	60.650446
2163.989667	60.423765	60.655450
2163.010906	54.819712	60.660455
2162.985517	58.687683	60.665460
2162.609160	47.988745	60.670465
2161.508958	60.180694	60.675470
2160.644926	52.632838	60.680474
2160.132447	54.373345	60.685479
2159.270421	58.851908	60.690484
2159.377195	53.782156	60.695489
2157.889977	62.171690	60.700494
2157.489812	59.969051	60.705498
2156.817534	55.462904	60.710503
2156.148289	60.792464	60.715508
2155.635275	53.329276	60.720513
2154.962877	59.053603	60.725518
2154.304891	59.880419	60.730522
2153.715662	57.516952	60.735527
2152.765304	56.647493	60.740532
2152.684377	51.840928	60.745537
2151.648250	53.612477	60.750542
2151.198053	60.131089	60.755546
2150.570140	51.167415	60.760551
2149.856917	63.589729	60.765556
2149.583739	50.901506	60.770561
2148.913366	50.462324	60.775566
2147.783707	55.380774	60.780570
2146.578453	52.550459	60.785575
2145.758200	62.218844	60.790580
2146.035174	50.127782	60.795585
2145.418269	52.115112	60.800590
2144.332826	66.594635	60.805594
2143.735882	53.402653	60.810599
2142.631964	55.128186	60.815604
2142.584408	56.211414	60.820609
2141.537355	61.474756	60.825614
2140.985964	58.300982	60.830618
2140.659947	56.083427	60.835623
2139.633466	58.418041	60.840628
2139.312009	58.076476	60.845633
2138.572182	54.443710	60.850638
2138.193231	64.078350	60.855642
2137.576352	55.414148	60.860647
2137.129766	59.661208	60.865652
2136.136516	59.973478	60.870657
2134.855664	64.587895	60.875662
2134.270918	59.310871	60.880666
2133.720909	57.220328	60.885671
2133.476712	65.888923	60.890676
2132.583067	59.560118	60.895681
2131.437722	56.450625	60.900686
2130.800752	50.051133	60.905690
2131.217975	53.063493	60.910695
2129.777672	66.676739	60.915700
2129.063163	57.993333	60.920705
2128.451960	55.210704	60.925710
2128.063681	57.068716	60.930714
2127.956822	58.336408	60.935719
2126.713929	55.712362	60.940724
2126.455025	57.207622	60.945729
2125.906928	54.772976	60.950734
2124.308309	58.127271	60.955738
2123.542531	60.065683	60.960743
2123.089096	58.448710	60.965748
2122.965863	61.956863	60.970753
2122.030482	67.539988	60.975758
2121.414060	66.439344	60.980762
2120.926542	54.392308	60.985767
2119.836861	58.632594	60.990772
2119.845152	52.867211	60.995777
2119.041112	64.529599	61.000782
2118.027305	61.684689	61.005786
2118.188444	62.614946	61.010791
2116.617393	58.186763	61.015796
2115.764085	52.346767	61.020801
2114.478703	68.480829	61.025806
2114.668012	59.330714	61.030810
2115.175243	51.308229	61.035815
2113.738289	54.438166	61.040820
2112.899419	59.980744	61.045825
2112.041113	57.357186	61.050830
2111.505739	58.926280	61.055834
2111.178956	57.967352	61.060839
2110.156913	60.157759	61.065844
2109.180325	56.190383	61.070849
2108.759712	62.597066	61.075854
2108.198088	58.183770	61.080858
2107.456413	51.316739	61.085863
2106.668337	57.702875	61.090868
2106.607979	52.494051	61.095873
2105.825986	55.939565	61.100878
2105.173026	62.649641	61.105882
2104.963125	62.687800	61.110887
2103.507925	62.888867	61.115892
2102.630806	61.265005	61.120897
2101.695484	63.818574	61.125902
2101.256533	61.674142	61.130906
2101.705297	55.018788	61.135911
2100.485234	57.638042	61.140916
2099.651470	53.048720	61.145921
2098.961968	56.856479	61.150926
2098.718757	54.084856	61.155930
2097.943876	50.580678	61.160935
2096.521687	61.686674	61.165940
2095.903102	56.500194	61.170945
2096.024881	51.197811	61.175950
2094.951026	54.934086	61.180954
2094.388677	52.952751	61.185959
2093.566486	59.722800	61.190964
2092.822633	46.863260	61.195969
2092.435069	57.809808	61.200974
2091.798332	55.701495	61.205978
2091.363518	57.992704	61.210983
2090.640881	51.876498	61.215988
2090.157643	47.920738	61.220993
2088.935116	54.416820	61.225998
2088.061181	54.367950	61.231002
2087.199038	48.373239	61.236007
2086.779834	59.006241	61.241012
2086.607464	49.866215	61.246017
2085.774954	52.900249	61.251022
2085.254889	55.867356	61.256026
2084.995504	51.305174	61.261031
2084.348938	59.122917	61.266036
2083.596339	51.435975	61.271041
2082.417196	56.854348	61.276046
2081.575438	61.397531	61.281050
2081.258754	48.998525	61.286055
2080.514443	53.228176	61.291060
2080.456960	50.576905	61.296065
2079.519511	64.712812	61.301070
2078.160362	60.186367	61.306074
2077.539998	50.917146	61.311079
2076.672500	54.382544	61.316084
2076.523588	49.211433	61.321089
2075.707728	52.179745	61.326094
2075.058072	52.828625	61.331098
2074.633486	46.594161	61.336103
2074.017177	56.277504	61.341108
2073.826857	49.281988	61.346113
2073.189007	59.011332	61.351118
2072.000385	55.721063	61.356122
2071.215692	45.982725	61.361127
2070.314030	62.401278	61.366132
2069.950557	45.710613	61.371137
2069.377246	49.826391	61.376142
2068.729306	47.916997	61.381146
2068.500580	48.975354	61.386151
2067.730968	54.652041	61.391156
2066.632232	45.622756	61.396161
2065.678257	50.453426	61.401166
2065.317249	47.596416	61.406170
2064.430982	47.013308	61.411175
2063.843111	48.775258	61.416180
2063.806660	48.741737	61.421185
2063.390166	44.086214	61.426190
2062.636222	52.390962	61.431194
2061.539249	49.521426	61.436199
2060.895289	52.918236	61.441204
2060.523230	48.017523	61.446209
2059.317626	46.794339	61.451214
2058.648849	47.063030	61.456218
2057.892676	44.364934	61.461223
2056.926076	55.247242	61.466228
2056.617401	47.720115	61.471233
2056.192208	58.155358	61.476238
2055.789563	54.486457	61.481242
2055.455064	57.883047	61.486247
2054.397855	60.033320	61.491252
2053.215636	51.659154	61.496257
2052.497050	58.491623	61.501262
2052.196113	58.056919	61.506266
2051.557382	57.352524	61.511271
2051.005319	58.214598	61.516276
2050.488718	56.744868	61.521281
2049.993354	47.544136	61.526286
2048.813027	48.890719	61.531290
2047.969850	53.993993	61.536295
2047.092209	58.047679	61.541300
2046.736131	49.042478	61.546305
2046.130688	53.718488	61.551310
2045.585053	58.660994	61.556314
2045.516733	49.886112	61.561319
2044.626968	53.528531	61.566324
2043.507901	49.239994	61.571329
2042.937083	51.614299	61.576334
2042.049182	59.350492	61.581338
2041.901875	54.936121	61.586343
2041.319180	59.018699	61.591348
2040.913965	46.770962	61.596353
2039.403700	61.164950	61.601358
2038.642902	52.462117	61.606362
2038.025587	56.375135	61.611367
2037.504841	59.999996	61.616372
2037.175291	51.574101	61.621377
2036.665418	47.504300	61.626382
2035.820295	49.393822	61.631386
2034.919315	50.062096	61.636391
2034.122620	59.435005	61.641396
2033.357843	48.655809	61.646401
2032.991400	53.527296	61.651406
2032.465854	57.558225	61.656410
2032.005593	49.787058	61.661415
2031.709391	57.908774	61.666420
2031.087446	53.213316	61.671425
2029.699055	52.306181	61.676430
2028.774970	51.065143	61.681434
2028.522778	48.290223	61.686439
2027.815328	57.231046	61.691444
2027.777995	46.014681	61.696449
2026.114668	47.494704	61.701454
2025.166624	50.627522	61.706458
2025.152481	39.995727	61.711463
2024.303797	49.260180	61.716468
2024.009473	44.533232	61.721473
2023.347426	54.900401	61.726478
2022.812539	58.096969	61.731482
2021.884499	46.619816	61.736487
2020.399528	54.315145	61.741492
2020.173709	47.948213	61.746497
2019.518546	51.045589	61.751502
2018.966440	48.393970	61.756506
2018.828433	48.723522	61.761511
2018.281364	52.855646	61.766516
2018.063560	43.749656	61.771521
2016.551412	54.455189	61.776526
2015.867364	46.825209	61.781530
2015.432643	49.939641	61.786535
2014.863227	55.365354	61.791540
2014.160976	42.742117	61.796545
2012.736242	55.159089	61.801550
2011.736780	52.988510	61.806554
2012.092600	50.148634	61.811559
2011.345538	57.192226	61.816564
2010.979935	50.219808	61.821569
2010.082015	50.241008	61.826574
2009.647984	47.950724	61.831578
2008.943541	44.326580	61.836583
2007.623314	54.496995	61.841588
2007.366093	45.611743	61.846593
2006.803936	43.218785	61.851598
2006.147245	46.839991	61.856602
2005.827544	49.289572	61.861607
2004.580479	50.783972	61.866612
2003.815690	42.763084	61.871617
2003.184802	51.169747	61.876622
2002.599962	59.359355	61.881626
2002.285572	48.761018	61.886631
2001.635977	54.819246	61.891636
2000.767182	48.391931	61.896641
1999.835690	47.369714	61.901646
1998.916946	50.849575	61.906650
1998.630806	50.718481	61.911655
1998.156856	53.197276	61.916660
1997.969864	48.831791	61.921665
1997.282079	54.512854	61.926670
1996.188929	47.840433	61.931674
1995.315721	45.641938	61.936679
1994.550433	52.234229	61.941684
1994.315912	46.583094	61.946689
1993.594512	43.701291	61.951694
1992.751879	49.082055	61.956698
1992.117269	47.536445	61.961703
1991.538750	51.227255	61.966708
1991.173835	42.035803	61.971713
1990.446621	43.600672	61.976718
1989.743997	48.009820	61.981722
1988.816153	41.565075	61.986727
1987.930362	37.196962	61.991732
1987.748862	47.084128	61.996737
1986.732863	46.419129	62.001742
1986.258004	47.828819	62.006746
1985.773699	37.864634	62.011751
1984.812107	49.388027	62.016756
1984.088811	40.051597	62.021761
1983.437874	50.770268	62.026766
1982.907292	54.552827	62.031770
1982.820086	47.503109	62.036775
1981.552345	51.800093	62.041780
1980.706216	41.909109	62.046785
1979.971402	45.042790	62.051790
1979.279824	50.333345	62.056794
1979.183362	47.913786	62.061799
1978.490121	56.981681	62.066804
1978.054993	45.844234	62.071809
1976.976076	56.037865	62.076814
1976.174690	50.437282	62.081818
1975.955780	48.116013	62.086823
1974.892747	56.192278	62.091828
1974.884609	49.629940	62.096833
1973.408008	48.489238	62.101838
1972.447444	47.925840	62.106842
1972.168613	46.194443	62.111847
1971.594730	58.014299	62.116852
1971.297776	49.289911	62.121857
1970.834408	52.782662	62.126862
1970.023444	46.710483	62.131866
1969.017406	49.931377	62.136871
1968.065281	55.417845	62.141876
1967.618120	46.272570	62.146881
1967.212803	45.141611	62.151886
1966.932317	45.306111	62.156890
1965.940697	39.242110	62.161895
1964.964743	50.796176	62.166900
1964.477427	40.491827	62.171905
1963.960889	38.758737	62.176910
1963.255961	52.488714	62.181914
1962.238855	43.735130	62.186919
1961.279119	43.906517	62.191924
1961.211118	41.603878	62.196929
1960.374920	42.525264	62.201934
1959.765574	41.748414	62.206938
1959.760441	38.776582	62.211943
1958.720428	47.229266	62.216948
1957.755627	41.329758	62.221953
1957.038120	39.084483	62.226958
1956.329990	49.572521	62.231962
1956.172510	39.406644	62.236967
1955.332205	48.474226	62.241972
1954.248192	46.596233	62.246977
1953.388433	48.199499	62.251982
1952.758330	44.465794	62.256986
1952.834463	43.638488	62.261991
1951.969946	53.089989	62.266996
1951.940134	47.425290	62.272001
1951.078416	41.995157	62.277006
1949.917265	50.561699	62.282010
1949.375390	42.199496	62.287015
1949.060055	46.988754	62.292020
1947.531206	43.353558	62.297025
1946.709008	45.728357	62.302030
1945.734649	48.794410	62.307034
1945.874385	48.046899	62.312039
1945.278110	48.225256	62.317044
1944.799823	46.262155	62.322049
1944.363224	46.274807	62.327054
1943.864463	39.009709	62.332058
1942.893655	42.360647	62.337063
1942.094301	52.125104	62.342068
1941.357706	45.096468	62.347073
1941.118797	43.719887	62.352078
1939.712669	52.181807	62.357082
1939.102361	39.212825	62.362087
1937.882568	50.345101	62.367092
1937.716136	45.006466	62.372097
1937.285576	49.053870	62.377102
1936.756476	48.964504	62.382106
1936.584386	45.311073	62.387111
1935.896376	54.896997	62.392116
1935.109764	50.423264	62.397121
1934.077860	49.983176	62.402126
1933.337011	46.330139	62.407130
1933.277530	45.543284	62.412135
1932.030318	58.209674	62.417140
1931.642691	43.574655	62.422145
1931.080566	44.078778	62.427150
1930.129082	46.459912	62.432154
1929.428843	43.932763	62.437159
1928.682398	53.803950	62.442164
1928.070094	47.061539	62.447169
1927.510388	47.051156	62.452174
1927.138498	44.288944	62.457178
1926.532063	46.825053	62.462183
1925.163986	42.934098	62.467188
1924.627014	36.050415	62.472193
1923.935605	46.485336	62.477198
1923.278197	53.003743	62.482202
1922.997887	46.766911	62.487207
1922.410299	54.589508	62.492212
1921.483622	45.143449	62.497217
1920.649543	40.691452	62.502222
1920.071641	43.871206	62.507226
1919.794492	47.257125	62.512231
1919.333989	57.300558	62.517236
1918.307747	45.943131	62.522241
1917.769650	50.822953	62.527246
1916.556531	50.854796	62.532250
1916.352369	45.736633	62.537255
1915.691242	53.556711	62.542260
1914.734116	55.243261	62.547265
1913.802826	53.487707	62.552270
1913.471281	53.521536	62.557274
1913.231250	48.276594	62.562279
1912.399557	53.430123	62.567284
1912.165073	47.299567	62.572289
1910.828573	55.255250	62.577294
1909.972158	54.680073	62.582298
1909.688666	48.293927	62.587303
1909.314863	54.759429	62.592308
1908.817584	56.076491	62.597313
1907.640725	49.497832	62.602318
1906.702626	52.490328	62.607322
1906.540397	42.717900	62.612327
1905.803365	52.903009	62.617332
1905.340987	45.188988	62.622337
1904.423748	47.280823	62.627342
1903.390942	52.915745	62.632346
1903.149859	43.029671	62.637351
1902.472118	43.552154	62.642356
1902.026903	44.914572	62.647361
1900.761841	41.194947	62.652366
1900.079519	42.413644	62.657370
1899.718173	42.565755	62.662375
1899.036108	50.289802	62.667380
1898.893559	42.018772	62.672385
1897.815764	49.509156	62.677390
1896.972203	57.749314	62.682394
1896.638001	43.708263	62.687399
1895.638749	52.433638	62.692404
1895.506731	46.994920	62.697409
1894.426379	49.005413	62.702414
1893.409493	46.905463	62.707418
1892.985064	45.615113	62.712423
1892.286000	49.716190	62.717428
1891.874542	41.926277	62.722433
1891.305524	45.590362	62.727438
1891.011014	47.187493	62.732442
1890.103631	43.247074	62.737447
1888.904136	50.531263	62.742452
1888.846372	42.787706	62.747457
1887.952146	43.975389	62.752462
1886.582924	47.999922	62.757466
1886.084120	42.979009	62.762471
1885.520709	53.833620	62.767476
1884.922972	37.815774	62.772481
1884.659998	41.737221	62.777486
1884.421981	49.791347	62.782490
1884.058313	49.762467	62.787495
1882.850538	50.260288	62.792500
1882.379020	38.349582	62.797505
1881.361407	46.242029	62.802510
1880.063596	40.450622	62.807514
1879.688352	35.440060	62.812519
1878.958407	43.854577	62.817524
1878.377407	42.585934	62.822529
1877.800104	46.987827	62.827534
1877.588326	47.231320	62.832538
1877.414411	37.060182	62.837543
1876.074687	44.117460	62.842548
1875.390374	46.022502	62.847553
1874.712304	42.230198	62.852558
1874.001186	46.571329	62.857562
1873.508252	45.241393	62.862567
1872.342674	50.796473	62.867572
1871.799797	44.391589	62.872577
1871.623689	45.692360	62.877582
1870.971471	43.446207	62.882586
1869.927550	48.750143	62.887591
1869.069968	57.817338	62.892596
1868.445818	46.866063	62.897601
1868.046163	45.084471	62.902606
1867.810925	45.837928	62.907610
1867.602804	42.440978	62.912615
1866.263755	46.731985	62.917620
1865.812362	41.345556	62.922625
1864.286800	47.815715	62.927630
1863.194810	51.531298	62.932634
1863.391280	39.197551	62.937639
1862.874642	49.424949	62.942644
1862.391194	50.055376	62.947649
1861.777908	53.986713	62.952654
1861.159521	50.000419	62.957658
1859.887785	43.782228	62.962663
1858.922918	48.359207	62.967668
1858.643187	52.701241	62.972673
1858.287973	47.473018	62.977678
1857.939100	44.530532	62.982682
1857.407249	44.660831	62.987687
1855.846276	48.580197	62.992692
1855.053386	36.119666	62.997697
1854.671110	42.487157	63.002702
1854.341620	44.616584	63.007706
1854.353853	43.509241	63.012711
1852.885344	41.332771	63.017716
1851.862417	40.058602	63.022721
1851.376641	49.904184	63.027726
1850.690059	52.918269	63.032730
1850.763570	36.580957	63.037735
1849.297724	42.942285	63.042740
1848.532713	47.129541	63.047745
1848.223210	41.529762	63.052750
1848.062737	42.968411	63.057754
1847.493338	38.078574	63.062759
1845.872677	46.219757	63.067764
1844.995018	39.601514	63.072769
1844.469610	43.184561	63.077774
1844.253961	39.351964	63.082778
1844.234873	35.002423	63.087783
1843.338230	45.271231	63.092788
1842.455035	44.559970	63.097793
1841.651938	38.912401	63.102798
1840.788098	39.559072	63.107802
1840.748881	36.291438	63.112807
1839.177182	45.465711	63.117812
1838.549052	26.345908	63.122817
1837.830619	45.790154	63.127822
1836.921671	46.596965	63.132826
1837.289414	33.818107	63.137831
1836.712661	43.263363	63.142836
1836.667924	44.606360	63.147841
1835.537241	50.305734	63.152846
1834.364354	49.241476	63.157850
1834.075938	46.160075	63.162855
1832.829298	52.343096	63.167860
1832.189351	48.666184	63.172865
1831.655947	44.406191	63.177870
1830.754026	49.018919	63.182874
1830.721662	45.385893	63.187879
1829.813333	46.574257	63.192884
1829.197706	34.856776	63.197889
1828.133439	43.273921	63.202894
1827.702262	44.985806	63.207898
1827.576742	42.939905	63.212903
1826.660777	42.585538	63.217908
1825.667126	36.657551	63.222913
1824.973115	44.225799	63.227918
1823.990698	51.959703	63.232922
1823.993405	45.882968	63.237927
1823.290665	52.921137	63.242932
1823.092634	43.094479	63.247937
1822.386504	39.003852	63.252942
1821.511782	44.421295	63.257946
1820.942317	37.910256	63.262951
1819.649084	49.774950	63.267956
1818.955684	44.570471	63.272961
1818.386237	49.937867	63.277966
1817.757376	47.082426	63.282970
1817.714507	39.972070	63.287975
1816.377843	50.725526	63.292980
1815.593569	51.193980	63.297985
1815.166932	49.210087	63.302990
1814.907655	53.976260	63.307994
1814.064461	46.734345	63.312999
1812.698725	51.524814	63.318004
1812.327321	44.715800	63.323009
1811.793541	48.645560	63.328014
1811.457754	49.197352	63.333018
1810.789482	46.654122	63.338023
1810.172522	50.844689	63.343028
1808.900467	45.784141	63.348033
1808.281442	46.858760	63.353038
1807.706115	44.302349	63.358042
1807.571572	39.685694	63.363047
1806.902068	50.924613	63.368052
1806.253111	42.924834	63.373057
1805.248574	43.063965	63.378062
1804.738479	47.439427	63.383066
1804.383300	34.223392	63.388071
1803.738664	47.224669	63.393076
1802.647615	43.939542	63.398081
1801.772102	43.850015	63.403086
1801.192531	44.636076	63.408090
1801.183979	44.355261	63.413095
1799.740508	49.475068	63.418100
1799.024530	45.460132	63.423105
1798.408420	47.813288	63.428110
1797.838885	50.931809	63.433114
1797.784488	37.521343	63.438119
1797.085466	47.249392	63.443124
1796.641021	39.169830	63.448129
1795.377988	45.644069	63.453134
1794.654530	49.867322	63.458138
1794.668200	37.191999	63.463143
1793.121961	47.955086	63.468148
1792.458516	44.480628	63.473153
1791.716597	46.038421	63.478158
1791.325878	47.302309	63.483162
1791.077094	33.730315	63.488167
1790.611358	41.669200	63.493172
1789.671908	41.585099	63.498177
1788.663896	44.661279	63.503182
1788.114270	43.949109	63.508186
1788.212206	42.493820	63.513191
1786.824953	40.834378	63.518196
1785.870591	34.602106	63.523201
1785.237351	44.849601	63.528206
1784.833752	46.885141	63.533210
1784.728055	36.133868	63.538215
1783.524109	43.330484	63.543220
1782.662376	38.802500	63.548225
1782.205714	46.796722	63.553230
1781.641917	48.824585	63.558234
1781.288949	40.479747	63.563239
1779.805959	45.713079	63.568244
1779.356812	43.586101	63.573249
1779.069997	38.244526	63.578254
1778.426235	40.080068	63.583258
1778.048605	33.453418	63.588263
1776.466491	42.531596	63.593268
1776.306312	39.265827	63.598273
1775.923757	36.980031	63.603278
1775.115431	44.191101	63.608282
1774.491011	37.390738	63.613287
1773.351572	47.698121	63.618292
1772.962303	39.332240	63.623297
1772.260681	36.286506	63.628302
1771.896620	36.651968	63.633306
1771.299660	38.939005	63.638311
1770.339975	45.929669	63.643316
1769.883921	38.673608	63.648321
1769.399873	45.681785	63.653326
1768.211287	41.057468	63.658330
1767.197835	31.954875	63.663335
1766.390902	43.382787	63.668340
1766.291223	35.420384	63.673345
1766.016038	34.391804	63.678350
1765.241091	39.903811	63.683354
1764.807508	31.778379	63.688359
1763.653759	43.863806	63.693364
1763.141793	35.026949	63.698369
1762.861118	39.823329	63.703374
1761.489009	43.108738	63.708378
1760.873974	39.068322	63.713383
1760.244827	48.280621	63.718388
1760.216440	38.023309	63.723393
1759.400321	42.158774	63.728398
1758.254343	37.529274	63.733402
1757.717191	41.235632	63.738407
1756.975531	33.285293	63.743412
1756.769658	29.225637	63.748417
1756.025672	39.820325	63.753422
1754.925841	35.369592	63.758426
1754.435001	34.603937	63.763431
1753.769645	42.424707	63.768436
1753.179554	39.421193	63.773441
1752.942222	42.376569	63.778446
1751.651720	41.627516	63.783450
1751.220408	38.254987	63.788455
1750.306281	40.218635	63.793460
1749.978772	35.948044	63.798465
1749.336022	35.818415	63.803470
1748.335297	43.911660	63.808474
1747.678997	38.677658	63.813479
1747.009591	43.299217	63.818484
1746.835642	37.176425	63.823489
1746.443674	48.647258	63.828494
1744.961946	46.249007	63.833498
1744.788609	42.330848	63.838503
1744.034130	44.521474	63.843508
1743.414362	37.756654	63.848513
1742.272249	41.221602	63.853518
1741.582637	46.474042	63.858522
1741.215693	38.186631	63.863527
1740.663883	37.929013	63.868532
1739.991102	29.573477	63.873537
1739.668048	32.974580	63.878542
1738.100915	41.249252	63.883546
1737.923408	28.650041	63.888551
1737.285022	39.502370	63.893556
1737.171814	32.680758	63.898561
1736.422981	40.136294	63.903566
1735.000059	46.986059	63.908570
1734.626121	33.060193	63.913575
1734.327474	47.657709	63.918580
1733.495010	40.502441	63.923585
1732.503150	39.078297	63.928590
1731.949853	39.872816	63.933594
1731.479625	34.262316	63.938599
1730.687630	40.863632	63.943604
1730.482100	37.592454	63.948609
1729.363277	39.695858	63.953614
1728.453393	40.441349	63.958618
1728.077943	31.333647	63.963623
1727.395125	40.776835	63.968628
1726.776765	37.615381	63.973633
1726.044024	45.159835	63.978638
1725.056136	42.172195	63.983642
1724.876353	35.550405	63.988647
1724.223058	38.433065	63.993652
1723.915419	32.915023	63.998657
1722.748694	32.001237	64.003662
1722.047419	35.050800	64.008666
1721.700818	31.038732	64.013671
1720.844669	44.245507	64.018676
1720.077433	34.058239	64.023681
1719.383327	40.648743	64.028686
1718.536075	39.144863	64.033690
1718.724925	33.073272	64.038695
1717.787033	35.081708	64.043700
1716.645305	36.392340	64.048705
1716.134230	34.587469	64.053710
1715.798712	45.697651	64.058714
1715.107554	31.593501	64.063719
1714.092875	38.670189	64.068724
1713.136649	29.730434	64.073729
1712.828344	30.886618	64.078734
1712.154715	34.016954	64.083738
1712.037956	23.228032	64.088743
1710.833452	37.802244	64.093748
1709.941746	38.694675	64.098753
1709.407956	38.826889	64.103758
1709.277804	41.454563	64.108762
1708.914891	37.191179	64.113767
1707.173973	37.887307	64.118772
1706.815024	37.006089	64.123777
1706.371915	33.575516	64.128782
1705.913348	41.063808	64.133786
1705.100070	35.725435	64.138791
1704.108049	43.593367	64.143796
1703.231605	36.430906	64.148801
1702.938436	38.445762	64.153806
1702.041354	41.302489	64.158810
1702.105164	33.940220	64.163815
1700.890457	42.838648	64.168820
1700.067430	22.926643	64.173825
1699.719239	30.782201	64.178830
1698.938670	40.341851	64.183834
1698.774746	34.752097	64.188839
1697.576440	36.973802	64.193844
1696.975340	35.990689	64.198849
1696.420088	39.324592	64.203854
1696.054778	39.366966	64.208858
1695.303081	37.724907	64.213863
1694.393749	40.455839	64.218868
1693.629504	32.827677	64.223873
1693.344860	28.832584	64.228878
1692.206458	39.149285	64.233882
1691.518740	33.759433	64.238887
1690.669133	41.071701	64.243892
1690.650275	35.783781	64.248897
1690.237236	36.887213	64.253902
1689.333100	36.797539	64.258906
1688.613973	36.501848	64.263911
1687.662922	38.108658	64.268916
1687.481029	35.380970	64.273921
1686.293652	34.940444	64.278926
1685.448045	40.613514	64.283930
1685.165017	33.569707	64.288935
1684.580667	40.420346	64.293940
1684.269500	38.500144	64.298945
1683.142229	42.686629	64.303950
1682.196467	48.839267	64.308954
1681.804698	35.256892	64.313959
1681.405072	44.834892	64.318964
1680.736452	41.222508	64.323969
1679.761147	42.143998	64.328974
1678.712783	34.359106	64.333978
1678.744700	30.917746	64.338983
1678.061729	40.939746	64.343988
1677.609677	36.189023	64.348993
1676.629052	31.448139	64.353998
1675.613480	35.280969	64.359002
1675.378510	32.973326	64.364007
1674.840438	37.909950	64.369012
1673.730058	39.745513	64.374017
1672.922201	35.844569	64.379022
1672.295763	41.522256	64.384026
1671.962767	25.829912	64.389031
1671.260213	35.563265	64.394036
1670.994775	30.041685	64.399041
1669.900151	30.554748	64.404046
1669.504030	31.120872	64.409050
1669.364259	26.495603	64.414055
1667.742130	34.843702	64.419060
1666.925742	32.667842	64.424065
1666.299024	33.182281	64.429070
1665.811249	39.478228	64.434074
1665.555241	27.186413	64.439079
1665.148843	33.338535	64.444084
1663.801616	30.947357	64.449089
1663.233927	33.313349	64.454094
1662.370532	44.885876	64.459098
1662.381693	37.255986	64.464103
1661.465757	35.927051	64.469108
1660.604806	33.185799	64.474113
1660.156238	35.116527	64.479118
1659.492059	34.299571	64.484122
1659.209027	34.215333	64.489127
1658.148544	46.894724	64.494132
1657.252582	40.347279	64.499137
1656.965770	27.867958	64.504142
1656.163992	38.027112	64.509146
1655.323711	40.272394	64.514151
1654.339136	41.745759	64.519156
1654.153144	36.539587	64.524161
1653.614272	37.180433	64.529166
1652.900899	35.936026	64.534170
1652.533232	40.967019	64.539175
1650.956817	36.590463	64.544180
1650.515653	36.723746	64.549185
1650.564019	39.603779	64.554190
1649.880366	41.481961	64.559194
1648.776014	29.471576	64.564199
1647.866510	41.655441	64.569204
1647.785720	31.455362	64.574209
1647.101531	38.541077	64.579214
1646.030709	37.014385	64.584218
1645.312460	31.339220	64.589223
1644.459907	39.770102	64.594228
1644.534378	42.472512	64.599233
1644.117786	44.156873	64.604238
1643.037890	37.662310	64.609242
1642.042842	32.628822	64.614247
1641.316205	47.191813	64.619252
1640.990989	41.072561	64.624257
1640.294614	40.420008	64.629262
1639.303833	37.074872	64.634266
1639.033923	29.667845	64.639271
1638.200747	39.423533	64.644276
1637.985652	35.844781	64.649281
1636.781664	39.933076	64.654286
1635.905243	37.728913	64.659290
1635.742649	38.984970	64.664295
1635.142691	42.283406	64.669300
1634.549178	33.320761	64.674305
1633.381164	34.197182	64.679310
1632.827378	38.801973	64.684314
1632.590292	26.680637	64.689319
1631.768010	38.733945	64.694324
1631.207450	36.736667	64.699329
1630.313981	37.914852	64.704334
1629.774756	42.350163	64.709338
1629.116788	38.583128	64.714343
1628.422617	36.550302	64.719348
1627.346571	35.024449	64.724353
1626.860045	35.874618	64.729358
1625.973398	39.880964	64.734362
1625.931638	31.811602	64.739367
1625.335986	41.770851	64.744372
1624.584287	31.937571	64.749377
1623.564846	33.432256	64.754382
1622.952213	44.761514	64.759386
1622.711211	37.349894	64.764391
1621.646859	38.791787	64.769396
1620.861924	34.973959	64.774401
1620.895880	37.173413	64.779406
1619.809964	35.062465	64.784410
1619.689941	28.088978	64.789415
1618.431881	36.842922	64.794420
1617.743975	38.519923	64.799425
1617.077380	32.284591	64.804430
1616.367950	39.710234	64.809434
1615.748696	27.372053	64.814439
1614.730347	36.056375	64.819444
1614.281914	33.621791	64.824449
1614.093811	37.318455	64.829454
1613.479649	43.525671	64.834458
1612.615078	31.079794	64.839463
1611.645600	41.987893	64.844468
1611.257017	37.621366	64.849473
1610.815200	34.551754	64.854478
1609.987217	42.931430	64.859482
1609.098658	34.991866	64.864487
1608.484937	39.314427	64.869492
1607.962568	32.079985	64.874497
1607.767273	27.313723	64.879502
1606.183388	26.871568	64.884506
1605.651838	25.435853	64.889511
1605.454649	34.794019	64.894516
1604.863867	31.875816	64.899521
1603.714576	30.990856	64.904526
1602.726893	29.580295	64.909530
1602.292570	35.815713	64.914535
1601.847500	33.968840	64.919540
1601.467288	25.082718	64.924545
1601.184643	30.831959	64.929550
1599.799599	34.151042	64.934554
1599.615599	26.036470	64.939559
1598.976194	34.342027	64.944564
1598.302410	34.756720	64.949569
1597.359143	22.339130	64.954574
1596.164662	30.029503	64.959578
1595.938918	24.561560	64.964583
1595.335388	22.899147	64.969588
1594.914043	25.125199	64.974593
1593.793418	27.788799	64.979598
1593.251834	32.252874	64.984602
1593.126171	26.360572	64.989607
1591.955000	33.774415	64.994612
1591.070723	28.888943	64.999617
1590.232131	29.143728	65.004622
1589.726722	21.930258	65.009626
1589.772065	23.110699	65.014631
1589.062561	29.601160	65.019636
1588.296625	28.503904	65.024641
1587.414696	24.468096	65.029646
1586.532436	30.314179	65.034650
1586.411119	20.346074	65.039655
1585.449855	35.315367	65.044660
1584.669358	30.694125	65.049665
1584.145958	32.649369	65.054670
1583.217950	34.116927	65.059674
1583.132602	25.259661	65.064679
1582.124406	32.649191	65.069684
1581.245992	18.970702	65.074689
1580.495603	24.370028	65.079694
1580.155128	24.711267	65.084698
1580.064243	25.497009	65.089703
1578.798990	30.049252	65.094708
1577.976088	28.505280	65.099713
1577.622174	27.352028	65.104718
1577.063257	22.558382	65.109722
1576.098451	21.746633	65.114727
1574.894517	24.656881	65.119732
1574.596730	27.188179	65.124737
1574.378608	24.592425	65.129742
1573.676709	27.795095	65.134746
1573.431714	29.682452	65.139751
1572.342234	27.264566	65.144756
1571.898441	28.618922	65.149761
1571.416803	21.720246	65.154766
1569.726272	31.656319	65.159770
1569.296560	22.309686	65.164775
1568.670343	31.450568	65.169780
1568.227713	33.560150	65.174785
1568.254441	30.449222	65.179790
1567.018937	28.816258	65.184794
1566.697129	28.408585	65.189799
1565.662433	33.018826	65.194804
1564.675903	30.879497	65.199809
1563.532536	25.248250	65.204814
1562.750913	35.006800	65.209818
1562.986951	26.480121	65.214823
1562.592645	32.234489	65.219828
1561.972318	24.373766	65.224833
1561.862471	29.542006	65.229838
1560.715700	27.229429	65.234842
1560.166201	30.130327	65.239847
1558.511789	34.887925	65.244852
1557.704916	31.095683	65.249857
1557.409996	24.339242	65.254862
1556.531975	31.533043	65.259866
1556.470418	23.509419	65.264871
1555.996172	29.852114	65.269876
1555.494095	25.893167	65.274881
1554.945066	21.239892	65.279886
1554.121784	34.845193	65.284890
1553.483972	26.671839	65.289895
1551.933632	38.142206	65.294900
1551.395407	27.759341	65.299905
1551.148472	27.647300	65.304910
1550.642392	35.400213	65.309914
1549.844974	29.217232	65.314919
1548.540636	35.299136	65.319924
1548.310239	26.376607	65.324929
1548.010234	30.475853	65.329934
1547.404886	30.621047	65.334938
1546.367232	13.063091	65.339943
1545.571839	16.965063	65.344948
1544.920100	23.080476	65.349953
1544.646970	20.200134	65.354958
1543.872233	27.172508	65.359962
1543.214382	23.821827	65.364967
1542.526291	25.069915	65.369972
1541.446224	23.732409	65.374977
1541.515628	24.036913	65.379982
1540.743158	19.480651	65.384986
1539.808422	15.322358	65.389991
1538.707884	25.670933	65.394996
1538.634762	18.943914	65.400001
1538.246007	14.512776	65.405006
1536.908996	27.160423	65.410010
1536.151377	26.997057	65.415015
1535.207280	32.070760	65.420020
1534.680889	33.832511	65.425025
1534.686420	27.854709	65.430030
1534.056895	27.868121	65.435034
1534.146564	9.952841	65.440039
1533.091450	23.366300	65.445044
1531.930385	23.071486	65.450049
1531.389130	21.765071	65.455054
1530.814625	30.246416	65.460058
1529.841086	25.021892	65.465063
1529.168833	27.350905	65.470068
1528.846556	28.406820	65.475073
1528.019282	23.927082	65.480078
1527.256352	31.255577	65.485082
1526.733586	20.699947	65.490087
1525.961950	22.494359	65.495092
1525.914569	26.113466	65.500097
1524.814740	21.806358	65.505102
1523.835869	27.844439	65.510106
1523.682514	29.655732	65.515111
1522.454516	18.475682	65.520116
1521.577232	20.502939	65.525121
1520.933442	20.982275	65.530126
1520.626506	25.051083	65.535130
1520.353206	17.502688	65.540135
1519.692724	32.665487	65.545140
1519.016662	30.221359	65.550145
1518.219228	25.577600	65.555150
1517.544225	24.661472	65.560154
1516.981378	23.054119	65.565159
1515.828393	30.696926	65.570164
1514.798705	23.271876	65.575169
1514.386913	20.746331	65.580174
1513.764866	22.051745	65.585178
1514.123584	21.118021	65.590183
1513.318046	28.793933	65.595188
1512.372131	28.729884	65.600193
1511.832135	23.755042	65.605198
1510.684888	21.516687	65.610202
1509.873304	24.019241	65.615207
1508.976366	21.594445	65.620212
1508.472376	23.280095	65.625217
1508.265592	26.139159	65.630222
1507.423540	34.237219	65.635226
1507.625631	15.190671	65.640231
1506.389925	30.260360	65.645236
1505.762797	18.710429	65.650241
1504.761934	20.798333	65.655246
1503.866578	27.889238	65.660250
1503.540525	19.141204	65.665255
1502.645508	25.106037	65.670260
1502.300734	22.872639	65.675265
1502.039301	25.497520	65.680270
1500.689003	28.807975	65.685274
1500.221671	21.202101	65.690279
1499.410640	28.576094	65.695284
1499.123800	25.994422	65.700289
1498.340074	19.481261	65.705294
1497.197618	25.130579	65.710298
1497.031723	27.252969	65.715303
1495.985597	30.576596	65.720308
1495.649126	27.026614	65.725313
1495.184781	24.287058	65.730318
1493.954751	28.418975	65.735322
1493.768287	22.998425	65.740327
1492.935342	22.419659	65.745332
1492.463122	22.884354	65.750337
1491.684582	27.923876	65.755342
1490.321028	28.363048	65.760346
1490.237743	12.099624	65.765351
1489.737293	24.754704	65.770356
1489.439851	23.904749	65.775361
1488.695301	20.550514	65.780366
1487.769969	33.875557	65.785370
1487.616593	13.923498	65.790375
1486.520144	23.669003	65.795380
1485.505541	30.543883	65.800385
1484.885429	29.106497	65.805390
1484.463937	28.921271	65.810394
1484.034750	20.416726	65.815399
1482.716296	30.676942	65.820404
1482.041234	26.978907	65.825409
1481.555239	25.892394	65.830414
1480.794002	29.153405	65.835418
1480.861521	16.660408	65.840423
1479.861819	20.997016	65.845428
1478.794295	30.709544	65.850433
1478.279204	24.401295	65.855438
1477.745013	27.056908	65.860442
1477.661230	24.047129	65.865447
1476.372300	37.732754	65.870452
1475.946422	23.004622	65.875457
1475.602256	33.057967	65.880462
1474.544847	38.728478	65.885466
1473.575530	22.689439	65.890471
1472.871704	25.181187	65.895476
1472.475089	26.687343	65.900481
1472.210824	23.695208	65.905486
1470.874031	31.313622	65.910490
1470.362421	30.387311	65.915495
1469.762349	28.027321	65.920500
1469.304640	25.348221	65.925505
1468.984782	21.693096	65.930510
1467.771881	31.424001	65.935514
1467.173127	27.083021	65.940519
1466.486802	32.445385	65.945524
1466.056882	26.383817	65.950529
1465.252250	24.975761	65.955534
1464.374119	22.568494	65.960538
1464.008765	29.807008	65.965543
1463.730821	28.835678	65.970548
1462.928588	28.807164	65.975553
1461.519646	32.882368	65.980558
1461.100489	30.510976	65.985562
1460.669388	22.516129	65.990567
1460.055223	28.459998	65.995572
1459.058635	30.168746	66.000577
1458.355661	30.228545	66.005582
1457.330815	36.067362	66.010586
1456.995773	21.750607	66.015591
1456.845841	34.089776	66.020596
1456.265798	26.435587	66.025601
1455.297103	35.861166	66.030606
1454.512417	33.661415	66.035610
1454.258518	25.624212	66.040615
1453.555654	31.795082	66.045620
1453.190870	33.841844	66.050625
1452.221545	23.653692	66.055630
1451.370860	32.215214	66.060634
1450.957641	33.375483	66.065639
1449.689993	37.022936	66.070644
1449.205576	29.340934	66.075649
1448.591149	23.896936	66.080654
1448.195476	32.190589	66.085658
1447.917730	23.475891	66.090663
1446.610756	29.947789	66.095668
1445.979667	26.670158	66.100673
1445.650683	28.184494	66.105678
1444.379810	34.915603	66.110682
1443.707639	23.366542	66.115687
1443.053816	30.835420	66.120692
1442.596416	29.066237	66.125697
1442.457541	15.309710	66.130702
1441.837528	27.734623	66.135706
1441.109297	21.875025	66.140711
1439.861494	28.041035	66.145716
1439.465734	23.396549	66.150721
1439.178624	28.895754	66.155726
1437.919752	25.643780	66.160730
1437.095109	17.345612	66.165735
1436.689073	28.280898	66.170740
1436.071333	24.193697	66.175745
1435.901194	29.731087	66.180750
1434.667924	37.662672	66.185754
1433.874901	25.796907	66.190759
1433.535567	38.664530	66.195764
1432.931590	26.226213	66.200769
1432.794230	27.665937	66.205774
1431.653235	30.638789	66.210778
1430.872176	22.515056	66.215783
1430.152847	26.343466	66.220788
1429.851825	32.977210	66.225793
1429.003313	24.091440	66.230798
1428.209616	32.642333	66.235802
1427.771025	24.913628	66.240807
1427.486539	21.478407	66.245812
1426.489428	24.321152	66.250817
1425.642107	20.525927	66.255822
1424.844404	18.948039	66.260826
1423.925955	17.465041	66.265831
1422.811936	25.231005	66.270836
1422.430809	21.576163	66.275841
1422.185352	30.793751	66.280846
1421.457121	35.069887	66.285850
1421.543386	22.845166	66.290855
1420.884237	26.053694	66.295860
1419.864441	25.892606	66.300865
1418.985363	21.596196	66.305870
1418.335022	26.454499	66.310874
1417.904028	20.990819	66.315879
1416.901334	30.519586	66.320884
1416.356183	22.667465	66.325889
1416.005408	21.728218	66.330894
1415.086928	24.123203	66.335898
1414.422084	14.162666	66.340903
1413.202333	16.242812	66.345908
1412.688284	26.189106	66.350913
1412.683489	24.622398	66.355918
1411.942531	24.541580	66.360922
1411.206505	23.857545	66.365927
1410.523711	26.768616	66.370932
1410.049175	31.151096	66.375937
1408.782616	19.340112	66.380942
1408.142128	25.564157	66.385946
1407.570231	19.597716	66.390951
1407.017560	22.570112	66.395956
1406.516816	22.372262	66.400961
1406.447601	24.185957	66.405966
1404.879670	27.250335	66.410970
1404.085322	18.267655	66.415975
1403.815116	30.083428	66.420980
1403.412833	30.481826	66.425985
1402.725282	20.064399	66.430990
1401.588482	26.402027	66.435994
1401.468317	15.561661	66.440999
1400.825185	27.712692	66.446004
1399.569266	27.360470	66.451009
1398.861898	23.285949	66.456014
1398.199635	38.857505	66.461018
1397.905479	22.709614	66.466023
1397.352683	29.670400	66.471028
1396.866021	23.163678	66.476033
1395.777327	22.199791	66.481038
1395.375332	24.067958	66.486042
1394.880833	20.710281	66.491047
1393.708855	35.515975	66.496052
1393.041868	20.219032	66.501057
1392.655978	29.517291	66.506062
1391.895764	37.555061	66.511066
1391.603668	28.912043	66.516071
1390.302809	33.753899	66.521076
1389.466042	28.643322	66.526081
1389.061483	30.677488	66.531086
1388.078267	28.468313	66.536090
1388.298666	23.251204	66.541095
1387.607610	20.751148	66.546100
1386.954985	22.421019	66.551105
1386.288815	24.652898	66.556110
1385.484008	31.672669	66.561114
1384.623007	26.510750	66.566119
1383.923906	31.860968	66.571124
1383.135136	25.832804	66.576129
1382.920214	16.335382	66.581134
1382.067468	30.509976	66.586138
1381.048383	30.310941	66.591143
1380.363481	34.138624	66.596148
1380.046367	34.115030	66.601153
1379.952880	27.178359	66.606158
1379.071008	32.477201	66.611162
1377.947062	20.246149	66.616167
1377.406663	26.630919	66.621172
1376.981496	25.627804	66.626177
1375.985568	25.336775	66.631182
1375.127797	28.468070	66.636186
1374.604417	32.167570	66.641191
1374.310072	29.483022	66.646196
1373.765024	32.950986	66.651201
1373.163703	26.232244	66.656206
1372.072645	31.617960	66.661210
1371.373937	22.739944	66.666215
1370.055664	30.536819	66.671220
1369.351916	22.446555	66.676225
1369.534680	24.923561	66.681230
1368.871962	31.405053	66.686234
1368.422143	29.737188	66.691239
1367.629172	28.956554	66.696244
1367.217015	21.386102	66.701249
1366.169190	24.967105	66.706254
1365.465107	26.771326	66.711258
1365.182927	31.260439	66.716263
1363.869741	29.564226	66.721268
1363.080298	22.230379	66.726273
1362.988370	17.939760	66.731278
1362.462991	36.586888	66.736282
1361.802094	29.130095	66.741287
1360.806481	29.143392	66.746292
1360.055627	22.003698	66.751297
1359.903515	24.067128	66.756302
1359.006525	33.743124	66.761306
1358.159019	28.337780	66.766311
1357.423921	34.775585	66.771316
1357.010843	33.011989	66.776321
1356.791807	34.176099	66.781326
1355.489425	39.306816	66.786330
1354.826662	32.230390	66.791335
1354.113520	37.239051	66.796340
1353.744192	38.442824	66.801345
1352.856634	33.263057	66.806350
1351.829583	36.091666	66.811354
1351.574967	28.176028	66.816359
1350.776993	30.126074	66.821364
1350.601806	35.978102	66.826369
1349.961373	24.419301	66.831374
1348.770239	37.611577	66.836378
1348.355198	21.394604	66.841383
1347.777393	29.110050	66.846388
1347.160058	31.851448	66.851393
1346.227172	26.174236	66.856398
1345.076137	32.924184	66.861402
1344.792568	31.469606	66.866407
1344.396806	30.969634	66.871412
1344.211532	26.542456	66.876417
1343.274655	26.317751	66.881422
1342.209556	27.020235	66.886426
1341.883937	29.407735	66.891431
1341.173267	39.502003	66.896436
1340.907043	35.480378	66.901441
1339.965138	31.679716	66.906446
1339.113029	37.163087	66.911450
1338.673154	28.054686	66.916455
1337.159848	34.297644	66.921460
1336.521727	22.446727	66.926465
1336.205949	26.783476	66.931470
1335.687879	30.759699	66.936474
1335.673052	28.182119	66.941479
1334.600954	30.842841	66.946484
1334.045573	25.247556	66.951489
1333.575045	28.303107	66.956494
1332.431673	29.208862	66.961498
1332.048007	29.143812	66.966503
1331.063483	38.240762	66.971508
1330.450526	28.219955	66.976513
1329.879651	31.780347	66.981518
1328.612599	35.516074	66.986522
1328.324967	24.673950	66.991527
1327.897952	31.058051	66.996532
1327.322488	24.746824	67.001537
1327.085839	25.224564	67.006542
1325.846721	29.082015	67.011546
1325.267496	20.998781	67.016551
1324.735885	27.464168	67.021556
1323.647534	34.918565	67.026561
1322.863808	26.741676	67.031566
1322.155226	35.061428	67.036570
1321.637066	26.776084	67.041575
1320.982462	28.157686	67.046580
1320.930401	31.482625	67.051585
1320.635549	28.487487	67.056590
1319.240486	39.210989	67.061594
1318.851133	25.989494	67.066599
1317.857497	32.190848	67.071604
1317.030789	33.060459	67.076609
1316.406276	34.405738	67.081614
1315.627077	33.149815	67.086618
1315.445877	30.090874	67.091623
1314.997285	36.172461	67.096628
1314.032426	36.852712	67.101633
1313.518734	29.326798	67.106638
1312.700904	31.749974	67.111642
1312.213581	32.920468	67.116647
1311.096167	33.416803	67.121652
1310.398519	31.493440	67.126657
1310.121642	27.486132	67.131662
1309.103386	41.149288	67.136666
1309.519420	24.940555	67.141671
1308.177292	31.700396	67.146676
1307.397092	33.278599	67.151681
1306.660949	32.960488	67.156686
1305.812736	39.074070	67.161690
1305.039804	31.529444	67.166695
1304.017292	34.235915	67.171700
1303.541965	30.993488	67.176705
1303.377308	27.834142	67.181710
1303.225259	29.892833	67.186714
1303.209416	27.613479	67.191719
1301.590064	28.607538	67.196724
1300.991507	31.257646	67.201729
1300.634488	24.618365	67.206734
1298.924048	30.228744	67.211738
1298.782580	18.133293	67.216743
1298.219107	21.891220	67.221748
1297.337850	33.252174	67.226753
1296.572546	21.702209	67.231758
1295.651140	24.698555	67.236762
1295.438170	25.543140	67.241767
1295.072576	28.799647	67.246772
1294.880906	28.549526	67.251777
1293.704417	30.217548	67.256782
1292.440604	28.906210	67.261786
1292.557910	26.285545	67.266791
1291.777756	27.297583	67.271796
1290.571518	30.433840	67.276801
1290.175134	29.232186	67.281806
1289.335691	26.571236	67.286810
1289.350761	26.714049	67.291815
1288.107978	31.005789	67.296820
1287.173866	25.278331	67.301825
1286.836897	27.593519	67.306830
1286.259831	27.079801	67.311834
1286.017981	24.317531	67.316839
1284.859121	32.431319	67.321844
1284.097917	27.863890	67.326849
1283.850346	26.293204	67.331854
1283.146554	35.126320	67.336858
1282.140789	28.282664	67.341863
1281.023559	35.090344	67.346868
1281.033897	29.931861	67.351873
1280.735610	22.914218	67.356878
1279.622467	31.651558	67.361882
1278.701981	33.417664	67.366887
1278.048759	37.366499	67.371892
1278.051077	33.136596	67.376897
1277.531396	31.142367	67.381902
1275.774977	35.138863	67.386906
1275.077205	33.664990	67.391911
1274.543986	32.871473	67.396916
1274.298596	30.516646	67.401921
1274.269189	30.713843	67.406926
1273.503266	36.500515	67.411930
1272.655165	31.519524	67.416935
1271.642139	35.164422	67.421940
1271.174672	38.880284	67.426945
1270.355947	26.192302	67.431950
1269.307419	38.767382	67.436954
1269.164367	29.741123	67.441959
1268.147504	36.744176	67.446964
1267.957134	26.474841	67.451969
1267.510309	23.869751	67.456974
1266.373440	33.799966	67.461978
1265.736974	28.652857	67.466983
1265.303551	33.804731	67.471988
1264.076288	27.366908	67.476993
1263.592307	25.594102	67.481998
1262.825583	33.303327	67.487002
1262.510287	24.063171	67.492007
1262.089919	27.527099	67.497012
1261.237712	26.375849	67.502017
1260.436417	19.783564	67.507022
1259.780542	23.513611	67.512026
1259.438992	25.386379	67.517031
1258.676769	30.049603	67.522036
1257.571396	34.130262	67.527041
1256.999551	28.378332	67.532046
1256.263644	24.980218	67.537050
1256.382899	19.361271	67.542055
1255.589245	28.661290	67.547060
1254.235373	32.784616	67.552065
1254.087159	28.487183	67.557070
1253.298496	32.113760	67.562074
1252.503538	27.206335	67.567079
1251.732190	27.051544	67.572084
1251.146884	34.249349	67.577089
1250.582856	31.028922	67.582094
1249.968688	21.501958	67.587098
1249.041155	22.392354	67.592103
1248.248182	32.591188	67.597108
1247.741907	29.148678	67.602113
1247.675128	24.270559	67.607118
1247.020149	16.134739	67.612122
1245.803392	20.819773	67.617127
1245.193293	29.467673	67.622132
1244.735538	23.585637	67.627137
1244.489738	21.305001	67.632142
1243.312970	25.893787	67.637146
1242.781634	18.689268	67.642151
1242.154715	21.053719	67.647156
1241.150468	24.813931	67.652161
1240.400684	31.345565	67.657166
1239.532522	27.140534	67.662170
1239.358143	28.852673	67.667175
1239.299668	30.721436	67.672180
1238.273701	31.271074	67.677185
1237.434738	24.604356	67.682190
1236.680530	23.533732	67.687194
1236.534944	17.775537	67.692199
1235.262965	33.966057	67.697204
1234.289559	25.349404	67.702209
1233.802396	16.710635	67.707214
1233.183660	27.302834	67.712218
1232.948867	23.334582	67.717223
1232.108743	31.563295	67.722228
1231.242134	31.939354	67.727233
1230.913282	27.140758	67.732238
1230.012565	28.099441	67.737242
1229.684374	20.435242	67.742247
1228.765674	21.852552	67.747252
1227.932207	21.278688	67.752257
1227.812314	18.362984	67.757262
1226.927265	24.280575	67.762266
1226.565857	18.343799	67.767271
1225.095723	25.157147	67.772276
1224.723645	32.901403	67.777281
1224.217415	20.170065	67.782286
1223.486940	31.234227	67.787290
1222.488968	26.308631	67.792295
1221.814992	20.957756	67.797300
1221.196068	26.304719	67.802305
1221.153577	25.155619	67.807310
1220.716321	29.462806	67.812314
1219.385294	20.661742	67.817319
1218.818786	29.491961	67.822324
1218.214565	32.523056	67.827329
1218.302900	17.620199	67.832334
1216.799041	30.168338	67.837338
1216.464673	24.432278	67.842343
1215.835969	24.690081	67.847348
1214.795863	35.699400	67.852353
1213.692560	25.939549	67.857358
1212.926965	31.095361	67.862362
1212.887259	20.120795	67.867367
1212.424755	29.694614	67.872372
1212.013640	27.462348	67.877377
1210.998208	21.071302	67.882382
1210.312654	32.098360	67.887386
1209.997476	24.105644	67.892391
1209.011467	31.733050	67.897396
1208.091081	25.935630	67.902401
1207.692100	27.771803	67.907406
1206.938562	30.285716	67.912410
1206.603069	23.173072	67.917415
1205.502532	30.506436	67.922420
1204.852415	25.892983	67.927425
1204.416218	20.570537	67.932430
1203.866315	32.372434	67.937434
1203.165568	20.359630	67.942439
1202.304735	30.320089	67.947444
1201.885272	18.349294	67.952449
1201.467424	25.742836	67.957454
1199.924110	25.434839	67.962458
1199.042169	24.411349	67.967463
1198.540071	28.615302	67.972468
1197.789446	24.919909	67.977473
1197.873559	23.250751	67.982478
1197.155254	30.409785	67.987482
1197.056313	26.943513	67.992487
1196.120915	28.431303	67.997492
1195.576984	27.494419	68.002497
1194.649219	16.186393	68.007502
1193.332892	27.853112	68.012506
1193.041918	28.106099	68.017511
1192.500379	26.678373	68.022516
1192.225389	23.277948	68.027521
1191.460918	16.935318	68.032526
1190.399094	25.603019	68.037530
1189.957606	19.642713	68.042535
1189.165375	23.602629	68.047540
1188.199701	28.050628	68.052545
1187.514766	20.236578	68.057550
1187.107602	23.966513	68.062554
1186.940712	15.674241	68.067559
1186.248972	23.787894	68.072564
1185.297028	19.924237	68.077569
1184.378059	19.067500	68.082574
1183.542765	26.639401	68.087578
1183.381927	16.038943	68.092583
1182.366457	28.083624	68.097588
1181.589818	23.435104	68.102593
1181.160352	26.714397	68.107598
1180.704916	25.731901	68.112602
1180.272564	21.550633	68.117607
1178.880912	21.694798	68.122612
1178.219363	24.619892	68.127617
1178.268061	16.159286	68.132622
1177.187489	24.722733	68.137626
1176.785836	22.015855	68.142631
1175.748704	23.341625	68.147636
1175.397329	24.831165	68.152641
1174.881166	18.698224	68.157646
1174.013332	22.078774	68.162650
1173.480455	18.225751	68.167655
1172.371338	28.355020	68.172660
1172.083712	24.846214	68.177665
1171.656244	27.010217	68.182670
1170.450320	28.712939	68.187674
1169.961704	17.625260	68.192679
1169.508804	21.576949	68.197684
1168.795677	26.711809	68.202689
1167.608243	24.109400	68.207694
1166.757570	29.589432	68.212698
1166.364502	20.773279	68.217703
1165.884855	26.642184	68.222708
1165.723704	24.646157	68.227713
1165.562935	20.202490	68.232718
1164.081050	23.967725	68.237722
1163.329212	28.616704	68.242727
1162.768873	30.924851	68.247732
1161.994396	25.656213	68.252737
1161.241370	25.269863	68.257742
1160.270507	28.521716	68.262746
1160.349875	24.041434	68.267751
1159.767820	21.271782	68.272756
1158.626524	29.859089	68.277761
1157.987769	27.044834	68.282766
1157.504095	27.222811	68.287770
1157.381360	29.951824	68.292775
1155.974497	31.680202	68.297780
1155.132782	21.200650	68.302785
1154.617868	25.122779	68.307790
1154.146944	29.047375	68.312794
1153.993356	21.218219	68.317799
1153.184909	31.362758	68.322804
1152.047830	31.772398	68.327809
1151.958966	19.938282	68.332814
1150.394467	31.985133	68.337818
1149.492707	26.574307	68.342823
1149.122609	30.990678	68.347828
1148.475605	27.658888	68.352833
1148.349353	19.532055	68.357838
1148.089225	31.740482	68.362842
1147.574270	27.666979	68.367847
1146.630288	32.687166	68.372852
1145.925756	31.201790	68.377857
1144.918269	27.192430	68.382862
1143.880472	36.728440	68.387866
1143.647121	30.801272	68.392871
1143.197617	35.339091	68.397876
1142.021190	30.708434	68.402881
1141.321617	25.481509	68.407886
1140.335917	38.962897	68.412890
1140.191968	30.255365	68.417895
1139.677336	31.340342	68.422900
1139.480988	32.267456	68.427905
1138.609868	22.890214	68.432910
1137.746658	33.925039	68.437914
1137.137184	19.898046	68.442919
1135.920403	26.037170	68.447924
1134.973819	25.774660	68.452929
1134.964979	19.769209	68.457934
1134.249924	28.086867	68.462938
1134.054915	14.539619	68.467943
1133.369149	32.049966	68.472948
1132.492097	26.736148	68.477953
1131.943198	17.500062	68.482958
1131.156888	24.187346	68.487962
1130.298741	25.128253	68.492967
1129.742753	26.024254	68.497972
1129.225099	27.385697	68.502977
1128.836774	28.980474	68.507982
1127.329582	31.186900	68.512986
1127.079164	22.512080	68.517991
1126.197059	28.027085	68.522996
1125.738106	19.562065	68.528001
1125.293719	23.905091	68.533006
1124.233129	23.351617	68.538010
1123.656628	17.997887	68.543015
1123.316086	27.555466	68.548020
1122.724290	29.188915	68.553025
1121.878127	24.504163	68.558030
1120.760867	33.251676	68.563034
1120.022284	28.127162	68.568039
1119.804715	38.829052	68.573044
1119.315384	24.732486	68.578049
1118.713775	23.822141	68.583054
1117.801212	28.234906	68.588058
1117.034566	20.813945	68.593063
1116.772543	25.392911	68.598068
1115.775527	30.741684	68.603073
1115.105260	16.804802	68.608078
1114.235182	30.986932	68.613082
1113.831887	26.056687	68.618087
1113.273915	19.469915	68.623092
1112.343587	30.302516	68.628097
1111.970143	28.102126	68.633102
1111.101222	33.086730	68.638106
1110.797787	26.945199	68.643111
1110.223726	31.676308	68.648116
1108.972806	33.222202	68.653121
1108.409886	21.083428	68.658126
1107.718431	29.340565	68.663130
1107.679168	30.824626	68.668135
1106.362364	30.103742	68.673140
1105.774068	30.277868	68.678145
1105.450067	25.423328	68.683150
1104.943793	27.735502	68.688154
1104.361959	20.616330	68.693159
1103.657108	28.650080	68.698164
1102.417565	27.366519	68.703169
1102.071889	24.854190	68.708174
1100.836484	31.021526	68.713178
1100.495297	29.807971	68.718183
1099.785678	27.659480	68.723188
1099.131151	26.727592	68.728193
1099.108460	30.505200	68.733198
1097.998715	42.457671	68.738202
1097.440675	24.238595	68.743207
1096.484332	28.565285	68.748212
1096.224144	29.797465	68.753217
1095.126508	29.041725	68.758222
1094.402164	34.922755	68.763226
1094.135418	26.794618	68.768231
1093.482308	39.322619	68.773236
1092.937316	33.738361	68.778241
1092.035043	30.904537	68.783246
1091.194810	32.456079	68.788250
1091.060024	25.510241	68.793255
1090.448479	33.609583	68.798260
1089.343694	41.885167	68.803265
1088.780128	35.204661	68.808270
1087.991866	39.605551	68.813274
1087.441673	29.481799	68.818279
1086.391335	28.765850	68.823284
1085.744387	25.784176	68.828289
1085.185511	31.943257	68.833294
1084.616488	31.688519	68.838298
1084.328635	21.947269	68.843303
1083.895429	29.469429	68.848308
1083.127420	34.354405	68.853313
1082.157613	27.475159	68.858318
1081.547353	30.571901	68.863322
1080.747997	33.788616	68.868327
1080.044187	32.949734	68.873332
1079.082128	39.266000	68.878337
1078.996417	35.805516	68.883342
1078.281573	36.133829	68.888346
1077.942692	35.244782	68.893351
1076.867251	38.428141	68.898356
1076.362341	33.223889	68.903361
1076.045603	33.033107	68.908366
1074.500321	35.901675	68.913370
1074.005114	30.949786	68.918375
1073.398745	32.561909	68.923380
1073.015279	28.271954	68.928385
1072.952915	23.060391	68.933390
1071.429550	31.371020	68.938394
1070.886582	27.207370	68.943399
1070.251772	36.447469	68.948404
1069.450940	36.392046	68.953409
1068.772904	28.960159	68.958414
1067.862906	29.347906	68.963418
1067.472066	27.538245	68.968423
1067.171178	35.110328	68.973428
1066.853530	28.859095	68.978433
1065.870672	23.869660	68.983438
1064.670259	31.654227	68.988442
1064.636725	26.967965	68.993447
1063.928954	31.007527	68.998452
1062.665591	33.970034	69.003457
1062.620801	24.549688	69.008462
1061.496672	35.693850	69.013466
1061.267288	33.926319	69.018471
1060.010712	30.999050	69.023476
1059.271387	32.460428	69.028481
1059.292929	22.761433	69.033486
1058.534188	31.858811	69.038490
1058.415644	25.875546	69.043495
1057.136387	31.829090	69.048500
1056.474701	30.838425	69.053505
1056.146401	25.823718	69.058510
1054.737869	35.333570	69.063514
1054.474583	27.058225	69.068519
1053.985498	30.367522	69.073524
1053.018281	27.337451	69.078529
1052.209285	26.105278	69.083534
1051.292494	29.477886	69.088538
1051.195944	24.415273	69.093543
1050.917602	31.493307	69.098548
1049.759179	28.755445	69.103553
1049.307890	27.109955	69.108558
1048.562697	32.566932	69.113562
1047.836046	24.251756	69.118567
1046.732412	28.794293	69.123572
1045.770947	23.970209	69.128577
1045.487001	17.768820	69.133582
1045.016369	20.553178	69.138586
1044.409451	18.828363	69.143591
1044.385823	21.547917	69.148596
1043.555960	25.242608	69.153601
1042.726504	23.349757	69.158606
1042.083428	35.344699	69.163610
1041.540490	28.817056	69.168615
1040.379025	31.429029	69.173620
1039.362374	20.658797	69.178625
1039.178666	18.827229	69.183630
1038.399849	29.873878	69.188634
1038.313281	27.750872	69.193639
1037.143335	25.202520	69.198644
1036.223627	33.764082	69.203649
1035.971013	33.023753	69.208654
1035.184398	33.505430	69.213658
1034.734420	25.586239	69.218663
1033.590001	30.463296	69.223668
1033.196273	27.570669	69.228673
1032.601427	25.058566	69.233678
1032.068327	24.219350	69.238682
1031.852864	34.417820	69.243687
1030.612329	30.609599	69.248692
1030.223967	23.333505	69.253697
1029.609659	23.566984	69.258702
1028.436798	25.543647	69.263706
1027.244392	29.765982	69.268711
1026.752054	36.278785	69.273716
1026.838673	30.040518	69.278721
1026.599057	20.211179	69.283726
1025.699568	29.982274	69.288730
1024.700890	24.503336	69.293735
1023.837220	30.430202	69.298740
1023.705264	29.877272	69.303745
1022.679395	28.277465	69.308750
1021.502881	30.276792	69.313754
1021.466253	28.426555	69.318759
1020.626903	36.120580	69.323764
1020.121748	37.194609	69.328769
1019.636377	28.831592	69.333774
1018.623666	36.589471	69.338778
1018.052421	29.526987	69.343783
1017.921638	32.806096	69.348788
1016.739992	32.060601	69.353793
1016.134010	21.012143	69.358798
1015.378923	39.233745	69.363802
1014.892451	37.543392	69.368807
1014.070075	28.289342	69.373812
1013.048089	31.491030	69.378817
1012.636714	18.708402	69.383822
1012.366514	32.230529	69.388826
1011.919913	21.795419	69.393831
1010.920360	32.102865	69.398836
1010.085275	32.806739	69.403841
1009.497607	22.055008	69.408846
1008.817032	28.241346	69.413850
1007.846087	25.727582	69.418855
1007.235118	22.915259	69.423860
1007.041110	30.531842	69.428865
1006.609864	21.125679	69.433870
1005.531552	35.702107	69.438874
1004.677649	26.385266	69.443879
1004.020926	31.314060	69.448884
1003.542249	24.094921	69.453889
1003.100345	28.365026	69.458894
1002.339781	30.099474	69.463898
1001.758175	18.924135	69.468903
1001.197967	29.466050	69.473908
1000.191126	27.284449	69.478913
999.495546	28.896588	69.483918
998.459090	28.047573	69.488922
998.281538	21.326186	69.493927
997.824266	25.882603	69.498932
997.356112	27.639919	69.503937
996.594791	19.991064	69.508942
995.569539	23.977068	69.513946
995.356192	26.695267	69.518951
993.969414	29.667979	69.523956
992.901095	35.471290	69.528961
992.786566	27.845687	69.533966
992.274584	38.793123	69.538970
991.674988	30.672227	69.543975
991.668362	33.777031	69.548980
990.269903	31.481114	69.553985
989.852771	32.501718	69.558990
988.990935	33.482685	69.563994
988.555420	18.808294	69.568999
987.704861	38.178983	69.574004
986.999355	38.124190	69.579009
986.742416	28.515242	69.584014
985.312538	36.568177	69.589018
984.798824	27.159368	69.594023
984.089315	36.923906	69.599028
983.623485	24.653024	69.604033
983.426242	30.995868	69.609038
982.857990	24.593704	69.614042
981.884451	30.012907	69.619047
980.565459	37.491505	69.624052
979.998037	32.336651	69.629057
980.492928	27.129474	69.634062
979.035960	35.260843	69.639066
978.241883	36.330386	69.644071
977.775491	27.429743	69.649076
977.289689	28.030741	69.654081
976.791010	27.615016	69.659086
975.408278	24.111743	69.664090
974.836379	23.906377	69.669095
974.383130	24.349222	69.674100
974.034594	25.401494	69.679105
973.466735	26.548590	69.684110
972.498344	27.377773	69.689114
971.989879	26.884754	69.694119
971.533621	27.544133	69.699124
970.525689	23.604313	69.704129
969.860244	29.546965	69.709134
969.146350	32.381083	69.714138
968.865594	23.449330	69.719143
967.699793	24.825620	69.724148
966.961553	27.860742	69.729153
966.371410	21.135620	69.734158
965.786928	30.096471	69.739162
965.696829	17.839936	69.744167
964.760331	23.926647	69.749172
963.962152	33.199063	69.754177
963.472938	20.379946	69.759182
962.467111	32.000505	69.764186
962.032605	25.876704	69.769191
961.478806	26.322935	69.774196
960.778484	29.809370	69.779201
959.905976	22.345386	69.784206
958.784282	33.517579	69.789210
958.146242	24.145910	69.794215
957.796772	27.918736	69.799220
957.314273	32.329356	69.804225
957.513754	22.359192	69.809230
955.850855	31.220393	69.814234
955.229082	25.837640	69.819239
955.034448	30.774922	69.824244
954.197040	26.789049	69.829249
953.602474	19.381774	69.834254
952.245596	24.324210	69.839258
952.147402	29.323420	69.844263
951.747716	33.938496	69.849268
950.560727	38.396561	69.854273
950.271460	16.293104	69.859278
949.598334	38.991516	69.864282
949.032131	24.095064	69.869287
947.444744	31.278894	69.874292
946.857574	35.102163	69.879297
946.288371	19.791430	69.884302
945.724560	27.414814	69.889306
945.711098	18.486270	69.894311
945.201653	23.978298	69.899316
944.242158	28.415933	69.904321
943.833628	22.205998	69.909326
942.664544	30.734722	69.914330
942.266591	29.031877	69.919335
941.298932	30.942809	69.924340
940.301198	24.318824	69.929345
940.258772	25.066907	69.934350
939.802622	29.451257	69.939354
939.309977	25.692820	69.944359
938.400332	29.296152	69.949364
937.523023	34.916113	69.954369
936.993527	27.917979	69.959374
935.310344	42.377785	69.964378
934.938859	32.323420	69.969383
934.392795	27.430126	69.974388
934.163148	28.864054	69.979393
934.012196	24.879346	69.984398
933.355543	28.953384	69.989402
932.560434	23.891553	69.994407
931.891153	28.451753	69.999412
930.789644	29.899835	70.004417
929.794786	23.384213	70.009422
928.889635	28.980219	70.014426
928.625308	33.217345	70.019431
928.149132	21.977940	70.024436
927.332097	25.304748	70.029441
927.273447	19.546950	70.034446
927.042533	27.270334	70.039450
926.396233	25.036122	70.044455
925.334213	26.421148	70.049460
924.312612	35.607696	70.054465
923.478955	19.998414	70.059470
922.897408	24.779633	70.064474
922.576677	26.185476	70.069479
921.421075	25.748138	70.074484
920.583569	22.214907	70.079489
920.308093	25.334103	70.084494
919.533255	28.226820	70.089498
919.310225	15.316474	70.094503
918.633203	21.751436	70.099508
917.372029	29.582000	70.104513
917.158369	19.893640	70.109518
916.748623	23.731258	70.114522
915.868688	22.961454	70.119527
915.031125	22.673792	70.124532
914.409037	21.773065	70.129537
913.739352	12.773907	70.134542
912.554695	25.373890	70.139546
911.935442	18.328547	70.144551
911.792499	33.339651	70.149556
911.140429	26.895650	70.154561
910.910967	19.400322	70.159566
909.971593	34.123408	70.164570
908.983102	28.756447	70.169575
908.448979	27.688749	70.174580
907.834599	31.320801	70.179585
907.117235	18.124827	70.184590
906.211303	30.719886	70.189594
905.843658	30.510417	70.194599
905.470655	27.851073	70.199604
904.552907	40.331320	70.204609
903.619789	22.632517	70.209614
902.820111	25.992843	70.214618
903.026687	20.705376	70.219623
902.204796	28.500732	70.224628
901.114694	35.402011	70.229633
900.379400	27.039377	70.234638
899.385460	33.761340	70.239642
899.263477	28.224943	70.244647
898.821015	27.614196	70.249652
897.609171	20.661587	70.254657
897.367749	23.860526	70.259662
896.696993	26.555325	70.264666
896.039928	25.299025	70.269671
894.768526	24.061643	70.274676
894.224098	24.388118	70.279681
894.301747	19.810339	70.284686
893.675060	27.260799	70.289690
892.951786	22.507690	70.294695
891.663078	27.015082	70.299700
891.184966	29.471054	70.304705
891.298085	20.889821	70.309710
889.751015	24.550455	70.314714
888.963587	23.147738	70.319719
888.410145	30.949264	70.324724
888.242027	27.557107	70.329729
887.549290	28.804526	70.334734
886.187137	24.050588	70.339738
886.033739	16.390187	70.344743
885.224264	21.688685	70.349748
884.894821	27.719812	70.354753
884.017122	15.159684	70.359758
882.937663	22.934529	70.364762
882.472747	16.634231	70.369767
882.173006	14.352763	70.374772
881.857097	19.784034	70.379777
880.990165	9.590918	70.384782
879.581874	23.858743	70.389786
879.419326	24.479279	70.394791
879.052559	24.911532	70.399796
877.594719	14.187949	70.404801
877.305835	14.125231	70.409806
876.757488	22.358053	70.414810
876.441664	22.081990	70.419815
875.621544	23.076856	70.424820
874.320053	24.189338	70.429825
873.667145	19.902882	70.434830
873.188678	22.989729	70.439834
872.954368	21.692963	70.444839
872.399728	20.213776	70.449844
871.174718	16.149270	70.454849
870.641238	11.216146	70.459854
870.008461	21.835855	70.464858
869.950479	16.968986	70.469863
868.984985	16.350020	70.474868
868.325222	26.217047	70.479873
868.128689	14.941045	70.484878
866.737323	19.920551	70.489882
866.284158	18.276973	70.494887
865.679321	18.917439	70.499892
865.025559	20.958220	70.504897
863.848211	20.615839	70.509902
862.839637	21.306370	70.514906
862.728793	20.076691	70.519911
862.125337	26.730206	70.524916
861.648291	23.994383	70.529921
861.404906	15.961933	70.534926
860.082481	22.263072	70.539930
859.495632	22.418100	70.544935
859.071735	29.923029	70.549940
858.125739	27.227150	70.554945
857.494875	16.384575	70.559950
856.478479	26.508650	70.564954
856.359802	24.100589	70.569959
856.064799	26.536885	70.574964
854.981190	33.463955	70.579969
854.329921	22.479536	70.584974
853.183768	19.140544	70.589978
853.039094	23.804930	70.594983
852.498494	31.008295	70.599988
851.543823	24.740217	70.604993
850.739644	19.206748	70.609998
849.924507	26.553161	70.615002
849.769205	30.542689	70.620007
849.411914	28.544789	70.625012
848.416366	24.573088	70.630017
847.633756	9.383110	70.635022
847.304315	23.002965	70.640026
846.676476	14.487630	70.645031
845.428271	20.423704	70.650036
844.563034	20.436954	70.655041
844.787915	14.637191	70.660046
844.167744	23.734629	70.665050
843.150758	22.466242	70.670055
842.295878	21.725595	70.675060
841.476827	18.295119	70.680065
841.207341	17.543303	70.685070
840.280220	24.346114	70.690074
839.717240	23.890186	70.695079
839.387611	21.039437	70.700084
838.388444	23.280290	70.705089
837.969922	17.765872	70.710094
836.620826	26.897329	70.715098
836.173497	23.395071	70.720103
835.954104	26.314525	70.725108
835.227915	23.944812	70.730113
835.024809	22.699857	70.735118
833.716810	27.407477	70.740122
833.230494	19.596634	70.745127
832.430435	17.923118	70.750132
831.151558	18.317622	70.755137
830.933536	13.578738	70.760142
829.720555	22.291115	70.765146
829.790708	15.968745	70.770151
829.634994	16.264903	70.775156
828.999981	18.119771	70.780161
828.168442	17.569391	70.785166
827.563971	16.039796	70.790170
827.052613	13.266865	70.795175
825.516904	15.698787	70.800180
824.597782	20.480136	70.805185
824.795041	9.251859	70.810190
824.359879	21.552787	70.815194
823.404597	18.366364	70.820199
822.926259	14.060024	70.825204
821.931214	19.555242	70.830209
821.955402	14.511286	70.835214
820.369277	8.277506	70.840218
819.845428	13.282958	70.845223
819.335773	17.915547	70.850228
818.251496	18.203383	70.855233
817.558714	13.207317	70.860238
816.856364	12.147493	70.865242
816.304881	15.544032	70.870247
815.871120	21.410406	70.875252
815.431508	27.446457	70.880257
815.309252	17.464433	70.885262
814.180486	27.415585	70.890266
813.380698	19.284042	70.895271
812.786318	19.339349	70.900276
812.070956	21.875678	70.905281
811.410508	20.753989	70.910286
810.714061	25.711223	70.915290
810.044393	16.819336	70.920295
809.082631	27.948767	70.925300
808.030579	29.865295	70.930305
807.854125	18.124033	70.935310
807.422006	23.408219	70.940314
807.116473	17.098340	70.945319
806.241135	26.561274	70.950324
805.256554	19.487381	70.955329
804.981250	21.442701	70.960334
804.266693	29.033327	70.965338
803.449385	18.949043	70.970343
802.832331	21.733091	70.975348
801.869674	21.244594	70.980353
801.581864	18.548053	70.985358
801.380831	25.421386	70.990362
800.297894	15.811498	70.995367
799.379036	24.171122	71.000372
798.805734	15.992494	71.005377
797.931241	14.311915	71.010382
796.755365	16.320700	71.015386
796.448144	15.710523	71.020391
796.005223	24.364991	71.025396
795.474260	20.404520	71.030401
795.433297	17.761731	71.035406
794.556583	26.933134	71.040410
793.498135	19.443627	71.045415
792.931953	19.775164	71.050420
792.138349	21.097014	71.055425
791.266051	16.153187	71.060430
790.560416	20.271322	71.065434
790.405653	15.465600	71.070439
789.763199	10.844753	71.075444
788.973709	11.552479	71.080449
788.167298	18.645187	71.085454
787.150914	21.429726	71.090458
787.080215	17.247747	71.095463
786.565781	13.768800	71.100468
785.557859	15.553724	71.105473
784.611922	12.279094	71.110478
783.938216	18.394991	71.115482
783.793265	17.371031	71.120487
783.569939	18.919086	71.125492
782.376783	21.198727	71.130497
781.739194	20.445589	71.135502
781.278243	17.347658	71.140506
780.286619	6.923692	71.145511
779.203554	14.530398	71.150516
778.444607	18.130291	71.155521
778.098969	8.073447	71.160526
777.902494	13.681262	71.165530
777.641614	14.366347	71.170535
776.782681	13.538054	71.175540
775.990085	15.957369	71.180545
775.214559	24.202714	71.185550
773.999051	20.696595	71.190554
773.404984	16.804527	71.195559
772.881629	18.220563	71.200564
771.989737	25.131333	71.205569
772.034304	11.563378	71.210574
771.266395	26.317539	71.215578
770.200894	18.598918	71.220583
769.897370	13.719105	71.225588
769.287832	20.249014	71.230593
768.521057	14.670197	71.235598
767.417639	19.707997	71.240602
766.925108	14.833040	71.245607
767.145300	22.164469	71.250612
765.747943	16.615072	71.255617
765.034460	19.152691	71.260622
764.081116	24.825806	71.265626
763.807696	15.973362	71.270631
763.275447	19.739031	71.275636
762.486547	16.051458	71.280641
761.770470	10.742133	71.285646
761.233592	27.121718	71.290650
760.693942	16.646301	71.295655
759.852602	19.759395	71.300660
758.978425	23.558998	71.305665
758.684782	16.789894	71.310670
757.653118	23.172530	71.315674
757.171578	21.574495	71.320679
756.304257	16.875908	71.325684
755.624579	19.201554	71.330689
755.939162	8.340978	71.335694
754.468387	17.922369	71.340698
753.764473	14.744847	71.345703
753.160045	16.743106	71.350708
752.236033	25.303849	71.355713
752.444444	20.012933	71.360718
751.143225	17.476160	71.365722
750.282452	21.546460	71.370727
749.949233	25.078585	71.375732
749.254145	17.878202	71.380737
749.114599	16.795033	71.385742
747.792650	20.248010	71.390746
747.412692	11.996040	71.395751
746.950960	18.950300	71.400756
745.755871	21.525172	71.405761
744.997758	21.652296	71.410766
744.327062	22.872587	71.415770
743.853530	20.391713	71.420775
743.436608	17.852939	71.425780
742.904206	18.240613	71.430785
741.932037	14.776201	71.435790
741.191489	27.450626	71.440794
740.816825	21.142302	71.445799
740.649301	14.018790	71.450804
739.526503	22.045025	71.455809
739.060154	11.188922	71.460814
737.809035	22.988944	71.465818
737.091104	13.226358	71.470823
736.463739	14.065993	71.475828
735.701121	24.821518	71.480833
735.620478	14.629445	71.485838
734.892343	29.662727	71.490842
734.136252	13.151747	71.495847
733.099985	15.603561	71.500852
732.502591	21.363524	71.505857
732.282877	13.835138	71.510862
731.792403	20.317711	71.515866
730.641240	9.324623	71.520871
730.116692	12.789432	71.525876
729.251630	20.449765	71.530881
729.326368	13.319225	71.535886
728.118942	31.089285	71.540890
727.118280	19.408296	71.545895
726.945885	10.995544	71.550900
726.361609	16.792844	71.555905
725.413911	17.415386	71.560910
724.177361	22.228381	71.565914
723.953475	16.695617	71.570919
723.497589	16.769898	71.575924
722.844150	20.567485	71.580929
722.790685	17.649131	71.585934
722.066122	18.676143	71.590938
720.934765	15.055725	71.595943
720.290070	15.557482	71.600948
719.251122	21.606959	71.605953
718.700187	9.848070	71.610958
717.801236	15.556693	71.615962
717.808667	14.144180	71.620967
717.373851	18.343800	71.625972
716.112705	17.062298	71.630977
715.575484	16.214346	71.635982
715.023042	15.457132	71.640986
714.397447	26.804314	71.645991
713.432148	21.927366	71.650996
712.591454	20.143660	71.656001
712.335603	17.118750	71.661006
711.501360	20.473592	71.666010
711.315909	15.108185	71.671015
710.418804	11.881008	71.676020
709.415456	22.469849	71.681025
708.828618	11.147211	71.686030
708.444841	8.224679	71.691034
707.717852	11.176068	71.696039
706.764900	14.983497	71.701044
706.231184	16.330229	71.706049
706.068360	12.085651	71.711054
704.710631	18.207966	71.716058
704.233801	12.855837	71.721063
703.750130	11.663452	71.726068
702.692043	13.364926	71.731073
702.956892	7.519372	71.736078
701.485205	12.494399	71.741082
701.176248	13.592445	71.746087
700.530357	8.593684	71.751092
699.844651	8.666713	71.756097
699.042240	4.883540	71.761102
698.274851	7.652119	71.766106
697.681760	10.843980	71.771111
697.517852	15.085627	71.776116
696.192319	21.603389	71.781121
695.634510	14.191924	71.786126
695.159915	15.434622	71.791130
694.824802	11.479267	71.796135
693.732511	17.922042	71.801140
692.663304	21.686484	71.806145
692.415495	19.571825	71.811150
691.933752	23.591254	71.816154
691.502735	11.600379	71.821159
690.331213	17.059082	71.826164
689.427179	15.843741	71.831169
689.355559	4.443810	71.836174
688.965908	3.051945	71.841178
688.068060	3.652369	71.846183
687.303699	9.994040	71.851188
686.703552	13.392042	71.856193
686.321306	6.380007	71.861198
685.029349	16.199477	71.866202
684.384310	8.161629	71.871207
683.934690	10.114751	71.876212
682.662200	22.754027	71.881217
682.057155	10.011808	71.886222
681.694994	16.044999	71.891226
681.224599	11.617574	71.896231
680.962611	11.151605	71.901236
680.234809	18.654468	71.906241
679.422157	10.073999	71.911246
678.348787	15.346758	71.916250
678.168169	18.245851	71.921255
677.831431	18.678082	71.926260
676.601330	21.807369	71.931265
675.763973	7.233354	71.936270
675.220761	16.320136	71.941274
674.764769	21.144487	71.946279
673.827373	14.137267	71.951284
673.146079	15.173172	71.956289
672.859653	10.782690	71.961294
672.189793	22.436561	71.966298
671.100583	23.857561	71.971303
670.121982	19.105760	71.976308
669.568472	19.616666	71.981313
669.390273	17.006776	71.986318
668.782995	14.564563	71.991322
668.603453	18.956943	71.996327
667.582391	12.764185	72.001332
666.648946	17.845923	72.006337
666.146220	10.338961	72.011342
664.883203	15.698696	72.016346
664.114734	16.041972	72.021351
664.003988	14.285559	72.026356
663.178160	17.121805	72.031361
663.140944	15.692747	72.036366
662.389960	13.767033	72.041370
661.704590	11.752020	72.046375
660.792903	20.550532	72.051380
660.315486	13.214591	72.056385
659.726969	4.752993	72.061390
658.467874	9.845585	72.066394
657.940483	8.718522	72.071399
657.638791	7.643833	72.076404
656.678726	14.675879	72.081409
655.738053	10.337541	72.086414
654.893869	16.852791	72.091418
654.554836	17.122954	72.096423
654.499614	10.080928	72.101428
653.860619	22.275541	72.106433
653.074088	14.697072	72.111438
651.890214	14.532460	72.116442
651.345135	13.551725	72.121447
651.222412	10.716949	72.126452
650.299898	14.298764	72.131457
649.530091	10.586114	72.136462
648.769001	22.221397	72.141466
648.527482	18.143905	72.146471
647.779735	17.640170	72.151476
646.552130	22.355576	72.156481
646.218944	12.555413	72.161486
645.523041	21.655477	72.166490
644.850977	21.328935	72.171495
643.902992	17.638351	72.176500
643.345715	23.395096	72.181505
643.026588	10.925922	72.186510
642.852344	10.444408	72.191514
641.961870	6.528614	72.196519
640.966974	6.294487	72.201524
640.110277	20.111845	72.206529
639.902314	13.625604	72.211534
638.794945	15.013237	72.216538
638.040836	14.299195	72.221543
637.867965	11.123880	72.226548
637.172772	13.625500	72.231553
636.458510	3.441307	72.236558
635.269645	11.052294	72.241562
634.555990	12.375653	72.246567
634.226012	13.275193	72.251572
633.757675	9.077699	72.256577
633.691489	11.214208	72.261582
632.290830	11.456309	72.266586
631.729503	10.386698	72.271591
631.146578	14.117878	72.276596
630.117054	11.235114	72.281601
629.502016	9.641019	72.286606
628.677664	14.894640	72.291610
628.397740	3.896919	72.296615
628.084038	8.706498	72.301620
626.877883	14.694317	72.306625
626.248020	16.346552	72.311630
625.598518	23.554670	72.316634
625.291304	11.096220	72.321639
624.880844	16.681343	72.326644
623.512409	20.982347	72.331649
623.026156	10.474822	72.336654
622.338707	16.247567	72.341658
622.088371	18.153192	72.346663
621.247005	13.879481	72.351668
620.418685	20.255013	72.356673
619.783276	13.598715	72.361678
619.489774	18.859269	72.366682
618.726502	13.570125	72.371687
617.806007	12.557717	72.376692
617.297630	17.604895	72.381697
616.797984	10.668344	72.386702
615.552997	21.033906	72.391706
614.844814	19.184974	72.396711
614.537300	14.663810	72.401716
613.797298	20.077479	72.406721
613.651048	18.810873	72.411726
612.395308	12.623975	72.416730
611.837069	11.340977	72.421735
611.140231	9.084942	72.426740
610.669997	3.536236	72.431745
609.875304	8.698400	72.436750
609.174853	14.413291	72.441754
608.677909	15.216416	72.446759
608.356628	10.478239	72.451764
607.217743	12.840783	72.456769
606.587874	2.225247	72.461774
605.769207	4.035294	72.466778
605.454335	4.487707	72.471783
604.524399	8.606911	72.476788
603.404114	13.858781	72.481793
603.070412	5.000209	72.486798
602.663282	7.501693	72.491802
602.380799	11.011555	72.496807
601.173380	3.739854	72.501812
600.369029	12.448740	72.506817
600.154119	0.447139	72.511822
599.319443	10.438253	72.516826
598.928056	0.272045	72.521831
597.987503	7.512320	72.526836
597.139796	13.069307	72.531841
596.752329	10.622070	72.536846
596.201995	20.414934	72.541850
595.429831	15.764338	72.546855
594.889586	10.898602	72.551860
593.909032	22.327561	72.556865
593.762699	3.847602	72.561870
592.582934	10.629213	72.566874
592.084680	12.266802	72.571879
591.536445	9.600731	72.576884
591.108043	18.323867	72.581889
590.105253	11.991034	72.586894
589.231977	23.478607	72.591898
588.783964	14.155664	72.596903
588.240531	16.019659	72.601908
586.912834	21.804494	72.606913
586.433289	23.664622	72.611918
585.990792	21.506863	72.616922
585.549168	8.722885	72.621927
585.240757	20.549446	72.626932
583.932710	25.142066	72.631937
583.562210	17.517865	72.636942
582.804072	28.324750	72.641946
582.430527	19.734307	72.646951
581.507714	22.598642	72.651956
580.722538	14.212544	72.656961
580.499127	11.417465	72.661966
579.694862	18.935682	72.666970
579.142612	15.601588	72.671975
578.000954	12.602658	72.676980
577.030935	20.656660	72.681985
577.195295	15.342794	72.686990
576.226510	19.674790	72.691994
575.289770	18.269149	72.696999
574.711879	15.350747	72.702004
574.037501	21.529876	72.707009
573.948818	13.750400	72.712014
572.710309	17.981846	72.717018
572.009058	9.683317	72.722023
571.731637	22.366005	72.727028
570.927604	15.340743	72.732033
570.564562	11.356741	72.737038
569.443083	25.034932	72.742042
568.908285	18.894085	72.747047
568.377985	17.728079	72.752052
567.812769	18.600437	72.757057
567.055554	13.251997	72.762062
566.086282	15.327332	72.767066
565.571559	16.008711	72.772071
565.063209	6.416255	72.777076
564.445749	12.029622	72.782081
563.754535	4.095373	72.787086
562.818041	20.432945	72.792090
562.498205	10.566019	72.797095
561.769941	2.334882	72.802100
560.710939	10.160192	72.807105
560.291051	7.368025	72.812110
559.690060	12.871532	72.817114
559.457064	4.181442	72.822119
558.300572	11.498707	72.827124
557.644666	9.039038	72.832129
557.214822	5.838428	72.837134
556.511138	14.372010	72.842138
555.872694	7.798225	72.847143
554.669861	7.220341	72.852148
554.148038	1.354998	72.857153
553.819403	2.990809	72.862158
553.101429	14.594003	72.867162
552.694591	7.570145	72.872167
551.740850	6.113603	72.877172
550.921047	7.652598	72.882177
551.022471	2.752483	72.887182
549.854262	9.320946	72.892186
549.136564	9.992079	72.897191
548.465270	9.206524	72.902196
547.818489	10.978171	72.907201
547.551962	-1.456764	72.912206
546.376042	8.776382	72.917210
546.236482	3.684405	72.922215
545.407351	8.863110	72.927220
543.868557	15.698776	72.932225
543.361650	7.763562	72.937230
542.437114	9.910631	72.942234
542.501384	12.299188	72.947239
542.238978	7.280396	72.952244
541.557393	17.795952	72.957249
540.994897	6.650860	72.962254
539.858316	12.561398	72.967258
539.427505	10.909595	72.972263
538.274976	9.992528	72.977268
537.564342	5.633370	72.982273
537.092400	4.294064	72.987278
536.426693	12.496730	72.992282
536.409864	7.519250	72.997287
535.681893	14.558520	73.002292
534.554682	21.841171	73.007297
534.091079	13.463796	73.012302
533.285914	7.246176	73.017306
532.292497	10.293670	73.022311
531.851438	15.522535	73.027316
531.137717	9.689339	73.032321
530.897150	6.963236	73.037326
530.222361	15.328209	73.042330
529.033028	15.098289	73.047335
528.720095	7.915968	73.052340
527.998358	16.733144	73.057345
527.874378	9.148543	73.062350
526.367059	16.340347	73.067354
525.765215	15.917492	73.072359
525.392863	10.715932	73.077364
524.747330	16.343242	73.082369
524.324078	-1.031235	73.087374
523.360573	14.463773	73.092378
522.692236	16.827096	73.097383
522.401206	14.929090	73.102388
521.222107	12.937570	73.107393
520.463970	9.372925	73.112398
519.812419	8.029116	73.117402
519.647508	11.002987	73.122407
518.815059	9.047718	73.127412
518.213965	12.497947	73.132417
517.541629	2.357589	73.137422
516.957102	7.998835	73.142426
515.843905	2.959451	73.147431
515.080044	5.013121	73.152436
514.153291	10.805084	73.157441
514.111510	3.953331	73.162446
513.512374	6.329287	73.167450
513.193208	9.264649	73.172455
512.318722	10.913298	73.177460
511.197231	23.457618	73.182465
511.148161	12.770091	73.187470
510.240699	13.555047	73.192474
509.664197	11.424960	73.197479
508.724536	10.166476	73.202484
507.960029	16.358396	73.207489
507.910442	2.734517	73.212494
506.902992	13.678897	73.217498
505.884110	15.292200	73.222503
505.484367	5.171502	73.227508
505.073291	9.742699	73.232513
504.763875	12.816866	73.237518
503.539897	20.767836	73.242522
502.813890	12.690905	73.247527
502.193090	13.244108	73.252532
501.207392	20.433260	73.257537
500.772722	14.271754	73.262542
499.964188	20.893337	73.267546
499.511583	19.591961	73.272551
499.321353	15.703450	73.277556
498.704369	16.077840	73.282561
497.515944	13.021741	73.287566
496.656668	20.294840	73.292570
496.250753	12.127494	73.297575
496.122548	13.469596	73.302580
494.767327	13.930051	73.307585
493.875151	9.077828	73.312590
493.363196	14.650746	73.317594
493.020663	10.903201	73.322599
492.868278	12.307504	73.327604
491.624435	18.895929	73.332609
491.109298	16.904312	73.337614
490.353794	19.519662	73.342618
489.984769	13.144263	73.347623
488.801289	16.349792	73.352628
487.820244	16.632365	73.357633
487.609549	14.019784	73.362638
487.077265	18.190804	73.367642
486.674020	5.400746	73.372647
485.802681	17.413182	73.377652
484.797888	12.793379	73.382657
484.560624	9.527409	73.387662
483.907739	17.899941	73.392666
483.204070	12.711745	73.397671
482.271567	15.759016	73.402676
481.730824	19.141289	73.407681
481.545530	10.292217	73.412686
479.970667	-1.541588	73.417690
479.070053	9.015173	73.422695
479.190026	6.310490	73.427700
478.387795	16.591372	73.432705
478.476656	6.471691	73.437710
477.194968	8.606292	73.442714
476.181465	9.840262	73.447719
475.961578	14.362080	73.452724
475.361140	8.420967	73.457729
474.645572	13.269348	73.462734
473.762726	9.355560	73.467738
473.168014	11.492689	73.472743
472.760933	10.155679	73.477748
471.235250	11.364009	73.482753
470.987546	6.595213	73.487758
470.222887	5.272592	73.492762
469.918112	11.350274	73.497767
469.675544	10.578444	73.502772
468.793946	7.922934	73.507777
468.054432	11.291141	73.512782
467.321837	10.381327	73.517786
466.619509	10.108544	73.522791
465.912140	15.619554	73.527796
464.854903	17.537044	73.532801
464.414166	8.345452	73.537806
464.049205	12.034054	73.542810
463.470629	11.479768	73.547815
462.537488	1.439333	73.552820
461.414636	12.315373	73.557825
461.400943	5.082239	73.562830
461.041252	13.814936	73.567834
460.317277	7.959745	73.572839
459.379730	5.866692	73.577844
458.874358	6.617569	73.582849
457.828536	0.618105	73.587854
456.783127	7.641728	73.592858
456.108358	2.882625	73.597863
455.862466	3.467576	73.602868
455.321547	6.031398	73.607873
455.131957	3.746638	73.612878
454.376161	15.160322	73.617882
453.789377	4.172106	73.622887
453.072097	7.443729	73.627892
451.861550	9.371456	73.632897
451.326006	-4.862570	73.637902
450.560513	5.779906	73.642906
450.382008	4.685619	73.647911
449.444177	5.604751	73.652916
448.267234	10.586574	73.657921
448.039494	10.339113	73.662926
447.107229	4.707934	73.667930
446.845376	5.948322	73.672935
446.172274	3.696441	73.677940
445.230605	9.233744	73.682945
445.034020	8.893006	73.687950
444.237277	8.058078	73.692954
443.405776	11.552917	73.697959
442.556489	11.014958	73.702964
442.020136	11.698231	73.707969
441.859104	7.696262	73.712974
441.271862	9.258166	73.717978
440.336195	3.272700	73.722983
439.609380	19.857599	73.727988
438.579938	11.573560	73.732993
438.053992	8.287356	73.737998
437.019023	15.831324	73.743002
436.374417	11.999447	73.748007
436.365294	14.579474	73.753012
435.637122	9.082947	73.758017
435.439129	2.219820	73.763022
434.110933	14.071654	73.768026
433.667259	11.961427	73.773031
432.898759	6.856123	73.778036
432.352019	6.601140	73.783041
431.522430	11.644326	73.788046
430.894898	10.489113	73.793050
430.414924	18.154403	73.798055
429.589874	16.338341	73.803060
428.741999	15.028992	73.808065
428.261754	6.384629	73.813070
427.308093	9.826393	73.818074
427.308103	9.725583	73.823079
426.118505	5.661984	73.828084
425.109322	16.409536	73.833089
424.835692	4.573454	73.838094
424.361160	8.981297	73.843098
423.827297	8.478247	73.848103
423.001546	5.306052	73.853108
421.955151	12.981161	73.858113
421.428915	5.892777	73.863118
420.860236	17.260884	73.868122
420.547794	12.190155	73.873127
419.882918	17.498854	73.878132
418.827548	20.220353	73.883137
418.634431	9.104762	73.888142
417.893738	10.328403	73.893146
417.040526	14.116885	73.898151
416.423611	8.127950	73.903156
415.646056	15.649834	73.908161
415.342845	6.526235	73.913166
414.076822	14.934969	73.918170
413.219820	14.587494	73.923175
413.016039	11.587447	73.928180
412.619922	16.214624	73.933185
412.391642	8.200357	73.938190
411.151158	11.415002	73.943194
410.338971	11.352139	73.948199
410.069410	11.363671	73.953204
409.260697	21.536788	73.958209
408.647306	15.839043	73.963214
407.921251	17.270101	73.968218
407.041600	11.643170	73.973223
405.986445	12.946885	73.978228
405.125670	17.774266	73.983233
405.135892	12.112780	73.988238
404.553689	19.288134	73.993242
404.408195	12.257362	73.998247
403.370680	11.648479	74.003252
402.493838	11.103885	74.008257
402.136724	10.585292	74.013262
401.079542	8.202227	74.018266
399.947094	10.827199	74.023271
399.764771	3.225106	74.028276
398.678156	12.628752	74.033281
398.622540	4.493932	74.038286
398.322661	13.923613	74.043290
397.674142	12.577777	74.048295
396.649552	15.385848	74.053300
396.098844	22.600343	74.058305
395.560534	6.696688	74.063310
394.107426	20.667480	74.068314
393.331862	21.026163	74.073319
393.282894	17.690772	74.078324
392.492822	17.115008	74.083329
391.970420	22.356854	74.088334
390.694276	19.164969	74.093338
390.268448	13.150322	74.098343
390.031050	17.149783	74.103348
389.657810	8.898408	74.108353
389.265778	8.677133	74.113358
387.787669	16.022058	74.118362
387.116334	11.532101	74.123367
387.026814	10.169736	74.128372
386.195928	17.591311	74.133377
385.045874	14.242135	74.138382
384.733824	13.039816	74.143386
384.140796	11.965854	74.148391
383.226324	11.629124	74.153396
382.233579	20.245076	74.158401
381.979409	11.269793	74.163406
381.278798	9.673630	74.168410
380.850213	12.836187	74.173415
380.695425	9.394654	74.178420
379.142345	19.585462	74.183425
378.755418	10.435783	74.188430
377.918310	13.111479	74.193434
377.676179	8.207760	74.198439
376.551830	4.428696	74.203444
375.966254	11.940496	74.208449
375.687664	5.911855	74.213454
374.872798	17.038485	74.218458
373.722148	14.118364	74.223463
373.828133	8.932079	74.228468
372.478153	13.801152	74.233473
372.444273	8.059961	74.238478
371.078812	15.965716	74.243482
370.335856	3.040586	74.248487
369.751831	10.720882	74.253492
369.023131	9.657505	74.258497
369.061022	5.431447	74.263502
368.692902	7.474138	74.268506
367.924819	7.864754	74.273511
367.350176	10.635829	74.278516
366.114257	9.405687	74.283521
365.397729	5.413397	74.288526
364.487585	7.998227	74.293530
364.143160	-1.065168	74.298535
364.084980	8.955229	74.303540
362.577263	6.442118	74.308545
361.942694	10.850241	74.313550
361.484218	11.699325	74.318554
361.157030	12.454944	74.323559
360.740613	6.564970	74.328564
359.280987	9.286255	74.333569
358.919892	6.918444	74.338574
358.132935	16.786888	74.343578
357.594685	0.403827	74.348583
356.729984	11.014824	74.353588
355.922808	10.659428	74.358593
355.533116	7.659053	74.363598
354.939350	17.184459	74.368602
354.440864	13.037569	74.373607
353.747492	8.119028	74.378612
352.751672	8.088601	74.383617
352.335488	4.982056	74.388622
352.110547	10.644879	74.393626
351.368340	10.988796	74.398631
350.689721	8.515461	74.403636
349.412244	20.931716	74.408641
349.173474	9.774525	74.413646
347.995747	11.663953	74.418650
347.327163	15.068200	74.423655
347.033327	9.934593	74.428660
346.451360	5.972908	74.433665
346.095199	2.374228	74.438670
345.023193	8.861206	74.443674
344.248999	-0.488528	74.448679
344.129575	5.723632	74.453684
342.744069	9.743629	74.458689
342.281847	3.977660	74.463694
341.525520	7.835883	74.468698
341.041604	10.794364	74.473703
341.038639	2.815172	74.478708
339.510365	7.061359	74.483713
338.895451	0.428704	74.488718
338.199685	4.211039	74.493722
338.116672	11.619097	74.498727
337.220728	4.108664	74.503732
335.964893	3.739618	74.508737
336.038554	5.994195	74.513742
335.338009	9.608552	74.518746
334.102423	11.406277	74.523751
333.476874	1.107139	74.528756
332.519028	5.071600	74.533761
332.468049	-0.135399	74.538766
331.766422	3.908082	74.543770
331.614114	7.941293	74.548775
330.900934	-1.468623	74.553780
329.780039	2.483975	74.558785
329.744896	-4.420856	74.563790
328.533703	10.653171	74.568794
327.364968	10.333329	74.573799
326.716918	12.501069	74.578804
325.991261	8.410894	74.583809
326.079791	7.945874	74.588814
325.598551	5.693415	74.593818
324.977886	8.487603	74.598823
324.396976	10.499555	74.603828
323.692845	9.108984	74.608833
322.259770	3.157112	74.613838
321.377139	12.167133	74.618842
320.962781	9.536567	74.623847
320.621934	6.984176	74.628852
320.243427	7.623393	74.633857
319.681691	2.284897	74.638862
318.585310	7.004762	74.643866
318.041076	14.169344	74.648871
317.649224	6.554922	74.653876
316.232363	7.711308	74.658881
315.677089	9.944692	74.663886
315.074874	13.336791	74.668890
314.890173	5.178397	74.673895
314.360045	5.233045	74.678900
313.239972	11.860168	74.683905
312.636739	6.283846	74.688910
311.822008	15.290935	74.693914
311.350302	11.671248	74.698919
310.504209	6.911110	74.703924
309.564294	9.953313	74.708929
309.653117	9.647526	74.713934
309.034482	11.332741	74.718938
308.088199	14.133096	74.723943
307.399856	13.096423	74.728948
306.827420	10.429550	74.733953
306.254076	7.284981	74.738958
305.233314	14.610675	74.743962
304.447860	12.138610	74.748967
304.038276	9.781690	74.753972
303.583635	11.923340	74.758977
303.224636	0.411573	74.763982
302.017320	13.059519	74.768986
301.341839	7.439519	74.773991
300.882320	7.079196	74.778996
300.181206	6.254306	74.784001
299.514752	10.497205	74.789006
298.492955	7.085053	74.794010
298.037200	3.513294	74.799015
297.799356	0.379914	74.804020
296.782634	0.441155	74.809025
296.032220	-3.662408	74.814030
295.453995	10.563232	74.819034
295.055995	4.315507	74.824039
294.513241	9.995868	74.829044
293.387460	13.133936	74.834049
293.016273	7.747727	74.839054
292.326979	5.170450	74.844058
291.579307	15.523104	74.849063
290.435290	5.469051	74.854068
289.677772	14.657846	74.859073
289.351430	11.295707	74.864078
289.000592	8.525707	74.869082
288.487648	8.695899	74.874087
287.754280	8.549547	74.879092
286.780476	6.222634	74.884097
286.429051	-8.649407	74.889102
285.863613	14.118551	74.894106
284.828342	4.037706	74.899111
284.206526	-0.430143	74.904116
283.549885	12.587376	74.909121
283.312189	1.220290	74.914126
282.011969	13.135539	74.919130
281.305355	12.123864	74.924135
280.748783	5.395189	74.929140
280.100176	13.691375	74.934145
280.040157	8.594632	74.939150
279.217537	16.227815	74.944154
278.291220	7.039554	74.949159
277.888812	5.071023	74.954164
277.121604	11.714458	74.959169
276.329718	9.328589	74.964174
275.272593	17.614195	74.969178
274.895716	16.592544	74.974183
274.639394	13.042618	74.979188
273.688623	11.860118	74.984193
272.866715	2.377663	74.989198
272.353500	9.240823	74.994202
271.901557	11.167572	74.999207
271.473875	10.381112	75.004212
269.963443	13.525306	75.009217
269.597052	5.922608	75.014222
269.156753	16.836584	75.019226
268.969886	13.294512	75.024231
267.633177	2.711342	75.029236
266.682566	11.263835	75.034241
266.620550	8.583426	75.039246
266.108180	3.058871	75.044250
264.993575	7.567186	75.049255
264.318535	3.413769	75.054260
263.721697	8.282699	75.059265
263.430542	8.026440	75.064270
262.510432	10.641281	75.069274
261.614012	6.461647	75.074279
261.213568	11.494826	75.079284
260.670251	16.374152	75.084289
260.282412	0.456035	75.089294
259.063083	2.166044	75.094298
258.063424	4.662672	75.099303
258.055027	-1.886854	75.104308
257.125108	8.837067	75.109313
256.145054	2.693171	75.114318
255.643079	1.902787	75.119322
254.946106	12.485495	75.124327
254.834467	-1.029092	75.129332
254.103856	9.155256	75.134337
253.318552	7.520590	75.139342
252.516757	9.837439	75.144346
251.811145	10.013119	75.149351
251.092287	6.128477	75.154356
250.624962	7.330669	75.159361
249.910899	0.521450	75.164366
249.161022	4.659379	75.169370
248.782974	9.852999	75.174375
248.198348	8.080685	75.179380
247.108953	6.794131	75.184385
246.564233	0.886789	75.189390
246.319009	-0.211038	75.194394
245.633074	-2.569627	75.199399
244.572129	3.196496	75.204404
243.538837	9.160074	75.209409
243.444833	1.739479	75.214414
242.971502	12.699722	75.219418
241.754222	6.587338	75.224423
241.344625	1.440666	75.229428
240.675290	7.387229	75.234433
240.274842	6.949690	75.239438
239.072744	6.955346	75.244442
238.513914	0.197082	75.249447
237.930092	2.843483	75.254452
237.205051	5.961849	75.259457
237.175267	2.117186	75.264462
235.803224	8.412324	75.269466
235.249615	9.234015	75.274471
234.982196	4.667105	75.279476
234.301900	5.608345	75.284481
233.221881	2.041493	75.289486
232.495088	9.090101	75.294490
232.192205	-2.380126	75.299495
231.728491	-0.982955	75.304500
230.629116	6.243323	75.309505
229.872813	5.427252	75.314510
229.211465	11.732109	75.319514
228.941243	4.003699	75.324519
228.581783	-0.318290	75.329524
227.276347	9.143950	75.334529
226.700617	5.171842	75.339534
226.157177	11.062069	75.344538
225.458667	-5.503553	75.349543
225.132543	-2.773646	75.354548
223.924226	5.619655	75.359553
223.919108	-3.417367	75.364558
223.249635	3.486477	75.369562
221.831403	7.579566	75.374567
221.266867	3.388045	75.379572
220.637335	14.762718	75.384577
220.563755	1.174256	75.389582
219.933667	7.827384	75.394586
218.953680	1.987862	75.399591
218.610432	-0.870071	75.404596
217.559699	9.540367	75.409601
216.653258	-3.139418	75.414606
215.859366	10.421984	75.419610
215.469233	2.509256	75.424615
215.234555	-2.108602	75.429620
214.340303	7.603498	75.434625
213.706356	-0.268782	75.439630
212.722420	-0.676379	75.444634
212.183397	-1.394612	75.449639
211.863540	-0.687455	75.454644
210.823083	8.461300	75.459649
210.087117	-2.585047	75.464654
209.296066	5.489415	75.469658
208.860168	2.600519	75.474663
208.456502	4.085897	75.479668
207.879940	8.918488	75.484673
206.885351	4.298766	75.489678
206.398302	13.960149	75.494682
205.913004	-0.683941	75.499687
205.165602	0.069299	75.504692
204.357221	7.842159	75.509697
203.733762	2.709088	75.514702
203.526763	8.154578	75.519706
202.123991	8.312098	75.524711
201.932205	1.848585	75.529716
200.950098	2.511504	75.534721
200.448012	5.289969	75.539726
199.392631	8.104600	75.544730
198.600057	1.877224	75.549735
198.453230	-3.409105	75.554740
197.350664	9.674783	75.559745
197.386957	7.806645	75.564750
196.526763	10.016121	75.569754
195.481917	4.956540	75.574759
195.211178	9.869694	75.579764
194.624654	6.370848	75.584769
194.498744	0.950290	75.589774
193.060913	5.495971	75.594778
192.196686	8.909365	75.599783
192.039455	3.312441	75.604788
190.958902	17.145071	75.609793
190.227711	8.925581	75.614798
189.376538	13.619022	75.619802
188.809598	3.995023	75.624807
189.079819	13.907856	75.629812
187.798868	15.298126	75.634817
186.844631	2.343682	75.639822
186.459011	8.752828	75.644826
185.821498	8.953941	75.649831
185.681193	6.178780	75.654836
184.463673	14.196659	75.659841
183.756625	-0.856792	75.664846
183.020737	4.285069	75.669850
182.586713	2.395717	75.674855
182.356385	-0.683650	75.679860
180.907781	4.295861	75.684865
180.685288	4.195830	75.689870
179.693611	10.930272	75.694874
179.323458	1.356910	75.699879
179.090313	9.358202	75.704884
177.916686	11.579808	75.709889
177.819295	-2.388065	75.714894
176.880238	8.775748	75.719898
175.678613	5.199925	75.724903
175.122869	2.203981	75.729908
174.398179	5.293921	75.734913
174.276898	2.167205	75.739918
172.989071	7.999493	75.744922
172.082543	5.182485	75.749927
171.798032	14.332163	75.754932
171.581531	18.164293	75.759937
171.307543	7.659341	75.764942
169.660624	10.213466	75.769946
169.248950	8.544490	75.774951
169.005867	4.413702	75.779956
168.181842	13.326106	75.784961
167.317245	2.692963	75.789966
166.524509	13.694674	75.794970
165.959998	14.142786	75.799975
165.854509	4.418413	75.804980
164.307616	13.854522	75.809985
163.854228	14.180833	75.814990
163.009114	11.798759	75.819994
162.508396	16.428447	75.824999
162.402032	11.126204	75.830004
161.257401	14.781446	75.835009
160.957336	7.327478	75.840014
160.260405	3.108195	75.845018
159.427663	11.083658	75.850023
158.826761	3.628770	75.855028
157.930370	9.097442	75.860033
157.467340	4.892909	75.865038
157.022080	9.638339	75.870042
156.573039	13.310416	75.875047
155.505235	8.248205	75.880052
154.465205	15.542328	75.885057
154.577445	1.869053	75.890062
153.126785	17.213149	75.895066
152.281062	13.380307	75.900071
152.015120	11.771681	75.905076
151.322629	10.172715	75.910081
150.960737	8.610929	75.915086
150.400851	15.754376	75.920090
149.775918	16.940714	75.925095
148.722226	11.605006	75.930100
148.215692	11.520304	75.935105
147.971864	6.720976	75.940110
146.671510	10.882046	75.945114
145.902246	12.474616	75.950119
145.658433	5.804929	75.955124
144.896712	10.200254	75.960129
144.691530	6.224282	75.965134
143.659062	11.460755	75.970138
142.980939	18.457469	75.975143
142.570103	15.023667	75.980148
141.403546	17.521720	75.985153
140.785566	6.999081	75.990158
140.232033	10.145323	75.995162
139.610787	12.617931	76.000167
139.342397	4.862437	76.005172
137.885947	13.763719	76.010177
137.473497	1.047784	76.015182
137.037114	2.334952	76.020186
136.360826	12.166870	76.025191
135.790617	9.688931	76.030196
134.692707	17.097951	76.035201
134.088824	6.905820	76.040206
133.745424	9.550179	76.045210
133.373681	6.908125	76.050215
132.544223	9.536942	76.055220
131.767562	17.509781	76.060225
131.435358	10.620788	76.065230
130.079272	9.802609	76.070234
129.155406	13.283885	76.075239
129.254842	10.943609	76.080244
128.253359	8.365697	76.085249
128.347409	9.238690	76.090254
127.215036	10.830814	76.095258
126.096218	11.067686	76.100263
125.905091	13.045915	76.105268
125.041757	17.604114	76.110273
124.153790	3.844312	76.115278
123.453135	14.210001	76.120282
122.655389	20.820498	76.125287
122.768006	12.103765	76.130292
121.950670	17.485724	76.135297
121.298278	12.246897	76.140302
120.417269	15.804925	76.145306
119.674625	23.043757	76.150311
119.891640	14.431807	76.155316
118.182400	15.278518	76.160321
117.616120	6.963372	76.165326
116.910336	14.021273	76.170330
116.556970	14.520887	76.175335
116.258934	12.800682	76.180340
115.109270	11.684656	76.185345
114.537199	9.689589	76.190350
113.965148	13.231470	76.195354
113.323536	12.739362	76.200359
112.421018	6.304034	76.205364
111.442187	7.926877	76.210369
111.366341	5.909457	76.215374
110.771006	8.890474	76.220378
110.223251	7.176974	76.225383
109.347951	7.140044	76.230388
108.001274	14.038358	76.235393
108.496230	12.108121	76.240398
107.384871	14.878098	76.245402
106.262638	14.353818	76.250407
105.851816	11.684882	76.255412
105.169620	18.336884	76.260417
104.588144	5.307270	76.265422
103.710726	17.189866	76.270426
103.119128	13.942600	76.275431
102.527914	10.734700	76.280436
102.091015	9.263734	76.285441
101.792054	5.285375	76.290446
100.871493	8.994801	76.295450
100.195373	13.896908	76.300455
99.658144	14.845334	76.305460
98.381937	12.174042	76.310465
97.596259	13.084813	76.315470
97.328021	15.736116	76.320474
96.759728	10.603740	76.325479
96.574892	9.912635	76.330484
95.410476	23.362837	76.335489
94.805502	13.855321	76.340494
94.195156	8.781695	76.345498
93.278624	8.937436	76.350503
92.537545	10.937131	76.355508
92.030084	14.427714	76.360513
91.612458	12.242436	76.365518
90.647749	13.095022	76.370522
89.571579	15.313743	76.375527
89.352163	8.304267	76.380532
88.713628	13.216153	76.385537
88.474158	8.160660	76.390542
87.460853	3.551863	76.395546
86.778654	17.764143	76.400551
86.291308	9.972607	76.405556
85.785614	14.530557	76.410561
84.802294	5.936557	76.415566
84.039819	18.788049	76.420570
83.388607	14.511033	76.425575
83.126495	11.014101	76.430580
81.670311	11.147091	76.435585
81.171824	4.193161	76.440590
80.252373	17.558564	76.445594
79.779677	11.095706	76.450599
79.580587	12.874925	76.455604
79.321521	11.572732	76.460609
78.730475	0.233657	76.465614
77.544769	9.703677	76.470618
76.891065	13.575569	76.475623
76.450410	7.413547	76.480628
75.373746	11.786573	76.485633
74.718392	8.904316	76.490638
74.310823	15.668652	76.495642
73.776545	10.445699	76.500647
72.653818	8.618889	76.505652
71.671715	19.340149	76.510657
71.442751	7.064921	76.515662
70.845137	13.146748	76.520666
70.473998	5.524353	76.525671
70.044229	4.533250	76.530676
68.768040	19.564118	76.535681
68.374041	5.794956	76.540686
68.027838	16.645049	76.545690
67.011736	20.215177	76.550695
65.988919	14.191731	76.555700
65.218545	14.448759	76.560705
65.188592	5.978707	76.565710
64.418982	16.208740	76.570714
63.300327	14.510601	76.575719
62.958440	7.716212	76.580724
62.365507	14.177358	76.585729
62.285048	9.303100	76.590734
61.027103	10.398015	76.595738
60.250618	15.629967	76.600743
59.697669	8.498637	76.605748
58.824722	11.569673	76.610753
58.804005	5.176673	76.615758
57.481110	13.880069	76.620762
56.701656	9.427964	76.625767
56.338599	12.485495	76.630772
55.683336	10.223000	76.635777
55.658837	4.617541	76.640782
54.333295	15.522892	76.645786
53.851577	9.271225	76.650791
53.229731	15.104596	76.655796
52.122274	21.299282	76.660801
51.436665	15.605282	76.665806
50.870766	11.464488	76.670810
50.443045	9.935296	76.675815
50.056386	11.083656	76.680820
49.250205	18.763164	76.685825
48.466641	12.575408	76.690830
47.793873	14.028032	76.695834
47.380391	10.096332	76.700839
46.584506	18.267808	76.705844
45.346032	17.271640	76.710849
45.267023	7.744919	76.715854
44.639384	16.234931	76.720858
44.048836	13.023786	76.725863
43.039351	3.749552	76.730868
42.093945	12.954171	76.735873
41.978209	12.731466	76.740878
41.469668	11.964253	76.745882
40.936257	14.276211	76.750887
40.056081	12.417040	76.755892
39.275631	13.951498	76.760897
38.906888	5.303660	76.765902
37.949887	10.491863	76.770906
37.418485	14.107704	76.775911
37.063547	8.031373	76.780916
35.518180	4.390595	76.785921
35.121789	9.842640	76.790926
34.452271	12.649416	76.795930
33.935789	19.014793	76.800935
33.872363	9.987082	76.805940
32.128687	13.980785	76.810945
31.678809	7.802898	76.815950
30.758025	11.334180	76.820954
30.520892	9.072816	76.825959
30.346467	14.989379	76.830964
29.299971	19.313457	76.835969
28.648904	9.037421	76.840974
28.134610	10.884264	76.845978
27.542805	10.303807	76.850983
26.522418	10.321589	76.855988
25.649960	18.535247	76.860993
25.072724	7.638705	76.865998
24.741185	12.500062	76.871002
24.212125	12.644494	76.876007
23.674919	12.777608	76.881012
22.583119	12.914020	76.886017
22.306598	7.949606	76.891022
21.341442	10.842964	76.896026
20.186315	11.807954	76.901031
19.915529	12.989879	76.906036
19.220747	13.411492	76.911041
19.103758	11.410100	76.916046
18.646349	16.091253	76.921050
17.472765	14.783537	76.926055
17.082632	17.011144	76.931060
16.128721	20.221271	76.936065
15.186339	17.712833	76.941070
14.397813	21.196218	76.946074
13.826571	6.851340	76.951079
13.589411	15.797917	76.956084
12.956430	20.245289	76.961089
12.399829	6.585662	76.966094
11.365573	14.815666	76.971098
10.451376	20.312460	76.976103
10.513058	5.850862	76.981108
9.641740	16.201213	76.986113
8.721199	7.232944	76.991118
8.047319	8.815072	76.996122
7.729729	15.462555	77.001127
7.183730	14.808562	77.006132
5.779036	11.679977	77.011137
5.330095	7.306067	77.016142
4.707745	14.855333	77.021147
4.377465	18.502182	77.026151
3.807647	13.185563	77.031156
2.614567	14.429441	77.036161