Fri Mar 05 18:48:15 2021

Number of Points = 14581

Depth (nm)	Load (N)	Time (s)
0.546035	97.510670	0.000000
0.483263	82.914781	0.005005
-0.506870	50.219733	0.010010
-2.373054	3.109132	0.015014
-6.340811	-10.633549	0.020019
-12.168648	-0.245335	0.025024
-16.437115	-9.248572	0.030029
-21.139830	1.173082	0.035034
-25.640183	-3.768747	0.040038
-29.277023	-13.560267	0.045043
-33.203215	-1.529384	0.050048
-36.663785	-8.073667	0.055053
-40.257374	2.128516	0.060058
-43.492228	-2.162020	0.065062
-47.121939	-2.292617	0.070067
-51.282973	3.906316	0.075072
-54.888607	-2.799306	0.080077
-58.990143	-0.091781	0.085082
-62.694267	-3.944725	0.090086
-66.293852	-11.953858	0.095091
-70.087174	-7.311672	0.100096
-73.713918	-7.146234	0.105101
-77.853564	-4.986112	0.110106
-81.508562	-3.598742	0.115110
-85.058723	-6.843853	0.120115
-89.037305	-2.930598	0.125120
-92.477067	-4.302537	0.130125
-96.735044	4.263184	0.135130
-100.606639	-3.052794	0.140134
-104.174367	-3.559050	0.145139
-107.952086	-1.213770	0.150144
-111.481281	-5.586558	0.155149
-115.003868	-2.578650	0.160154
-118.736549	-5.168536	0.165158
-122.277188	-12.717052	0.170163
-126.648137	-11.429846	0.175168
-130.345722	-19.883708	0.180173
-134.519286	-6.792917	0.185178
-138.625268	-1.041021	0.190182
-142.060289	-11.354998	0.195187
-145.905565	0.114361	0.200192
-149.330014	-8.687413	0.205197
-153.041329	-0.311333	0.210202
-156.832404	-3.965750	0.215206
-160.578384	-12.962203	0.220211
-164.496759	-4.480528	0.225216
-167.749743	-7.533238	0.230221
-171.806624	0.506928	0.235226
-175.735470	1.950754	0.240230
-178.899067	-10.495950	0.245235
-183.108837	9.255470	0.250240
-186.846936	1.754327	0.255245
-190.896472	0.777884	0.260250
-194.423686	-3.267089	0.265254
-197.865081	-1.740167	0.270259
-202.403963	-0.848650	0.275264
-205.416804	-8.020799	0.280269
-209.537692	-7.158129	0.285274
-213.249554	4.586508	0.290278
-216.483240	-3.736255	0.295283
-220.739209	-0.838234	0.300288
-224.270383	-11.226625	0.305293
-228.219290	-2.892943	0.310298
-232.247267	-5.079129	0.315302
-235.992367	-6.031544	0.320307
-239.677957	2.725335	0.325312
-243.151859	-6.271833	0.330317
-246.984953	-6.380707	0.335322
-250.949717	-1.311912	0.340326
-254.463263	-10.108766	0.345331
-258.132896	-1.367026	0.350336
-261.806047	0.550215	0.355341
-266.242157	2.887287	0.360346
-269.753032	4.196741	0.365350
-273.207928	0.827896	0.370355
-277.261080	11.780280	0.375360
-280.653070	-1.687967	0.380365
-284.715712	7.988606	0.385370
-288.498744	-2.160791	0.390374
-291.995753	-0.047694	0.395379
-296.037314	8.977404	0.400384
-299.669997	-2.071186	0.405389
-303.491870	4.211219	0.410394
-307.373478	-4.648228	0.415398
-310.955719	-4.292419	0.420403
-315.229082	3.711572	0.425408
-318.725766	-8.363213	0.430413
-322.533139	0.157758	0.435418
-325.936545	6.978945	0.440422
-329.560769	-10.719386	0.445427
-333.461965	0.188319	0.450432
-337.139034	-6.016597	0.455437
-341.132012	-3.319625	0.460442
-345.139539	-2.998371	0.465446
-348.377873	-6.776992	0.470451
-352.362456	0.933375	0.475456
-356.157491	-1.624105	0.480461
-360.130680	1.478171	0.485466
-363.619893	0.795763	0.490470
-367.466659	-0.373604	0.495475
-371.730130	2.786075	0.500480
-374.743753	-8.430611	0.505485
-378.511572	0.401095	0.510490
-382.535120	-4.027971	0.515494
-386.012063	-6.418570	0.520499
-390.346511	-1.791998	0.525504
-393.789017	-5.632573	0.530509
-397.500763	-9.620964	0.535514
-401.175663	-5.342535	0.540518
-404.856246	0.324528	0.545523
-409.107411	0.192781	0.550528
-412.527875	-5.567285	0.555533
-416.670541	4.860287	0.560538
-420.013431	-5.035891	0.565542
-423.672800	-8.586326	0.570547
-427.735003	-3.988969	0.575552
-431.570637	-6.897811	0.580557
-435.320519	-5.578336	0.585562
-438.727986	-0.495731	0.590566
-442.524737	0.854894	0.595571
-446.594921	2.446308	0.600576
-450.101412	-3.006652	0.605581
-453.652231	-6.293678	0.610586
-457.579211	12.359602	0.615590
-461.621509	-4.245148	0.620595
-465.331603	10.595126	0.625600
-468.998094	-4.833293	0.630605
-472.996026	0.354695	0.635610
-476.755236	1.622108	0.640614
-480.121198	-0.491186	0.645619
-483.862084	6.497651	0.650624
-487.864115	0.149331	0.655629
-491.846536	6.050811	0.660634
-495.369626	-3.138385	0.665638
-499.150171	-2.977705	0.670643
-503.166768	-4.979165	0.675648
-506.745680	-6.526976	0.680653
-510.528867	3.046972	0.685658
-513.902889	7.086706	0.690662
-517.775496	-8.471132	0.695667
-521.788716	6.159013	0.700672
-525.311602	-8.260916	0.705677
-529.335777	4.890231	0.710682
-533.107369	-5.804625	0.715686
-536.590095	-4.456702	0.720691
-540.567006	2.703959	0.725696
-544.230887	-7.345761	0.730701
-547.792104	-4.529758	0.735706
-551.978857	-4.371918	0.740710
-555.436796	1.936317	0.745715
-559.343195	2.598166	0.750720
-562.878602	-2.369033	0.755725
-566.822264	-8.765958	0.760730
-570.599437	-0.769834	0.765734
-574.482060	-9.660194	0.770739
-578.259075	-0.341023	0.775744
-581.922880	-12.588959	0.780749
-585.576577	-5.615480	0.785754
-589.417980	-13.667151	0.790758
-592.783267	-3.825531	0.795763
-597.149429	1.475101	0.800768
-600.911977	-8.908846	0.805773
-604.667211	0.482580	0.810778
-608.522268	-5.672964	0.815782
-611.591968	-4.698422	0.820787
-615.404187	-4.251799	0.825792
-619.148624	-3.226221	0.830797
-623.339742	-0.358357	0.835802
-627.174565	-1.967601	0.840806
-630.691956	-15.494097	0.845811
-635.095213	3.743300	0.850816
-638.409528	-5.409638	0.855821
-641.917187	-8.676463	0.860826
-645.702921	-6.516726	0.865830
-649.287090	-15.058823	0.870835
-653.593788	2.406454	0.875840
-657.268641	-4.619891	0.880845
-660.935819	-4.712033	0.885850
-664.509880	-7.072507	0.890854
-667.788275	-10.615621	0.895859
-672.117711	1.732968	0.900864
-675.950622	-11.642116	0.905869
-679.882533	-3.674721	0.910874
-683.995375	-2.352054	0.915878
-687.335817	-8.062993	0.920883
-691.090244	1.412010	0.925888
-694.718654	-10.584351	0.930893
-698.190387	-8.329628	0.935898
-702.210906	-11.072862	0.940902
-705.960488	-8.289605	0.945907
-709.908879	-7.101982	0.950912
-713.684282	-2.884294	0.955917
-717.240985	-2.366377	0.960922
-720.877619	-5.700781	0.965926
-724.621090	-7.682431	0.970931
-728.472380	-4.354607	0.975936
-732.473346	-5.870895	0.980941
-736.328409	2.300353	0.985946
-739.946303	-0.414123	0.990950
-743.609029	-1.270091	0.995955
-747.420632	5.320436	1.000960
-751.020474	-0.978157	1.005965
-754.921608	-0.649564	1.010970
-758.432295	-3.154063	1.015974
-762.390431	-5.631199	1.020979
-766.202564	7.500621	1.025984
-769.631033	-7.541121	1.030989
-774.006625	-8.409262	1.035994
-777.739822	-0.342584	1.040998
-781.532705	-10.792335	1.046003
-785.329903	1.401992	1.051008
-788.643577	1.988405	1.056013
-792.522761	-5.935459	1.061018
-796.242718	-1.187189	1.066022
-799.333648	-10.377163	1.071027
-803.861269	-0.019896	1.076032
-807.714014	-3.185580	1.081037
-811.539848	-0.374200	1.086042
-815.170991	3.005307	1.091046
-818.838784	-2.888079	1.096051
-822.976770	2.750220	1.101056
-826.222824	-3.292569	1.106061
-829.976574	-3.476265	1.111066
-833.875780	1.206100	1.116070
-837.708290	1.821903	1.121075
-841.519272	4.302953	1.126080
-845.223027	5.014880	1.131085
-848.914120	-7.173055	1.136090
-853.206522	-9.949834	1.141094
-856.103377	-9.710657	1.146099
-860.016383	1.144544	1.151104
-863.940313	-3.124567	1.156109
-867.986703	9.259535	1.161114
-871.661710	-0.584441	1.166118
-875.016182	-5.890738	1.171123
-879.228026	4.118142	1.176128
-882.722764	-2.745821	1.181133
-886.032618	-2.945201	1.186138
-890.156872	-5.058093	1.191142
-893.871310	-14.222363	1.196147
-897.993796	-11.286147	1.201152
-901.692687	-14.268113	1.206157
-905.445056	-9.549189	1.211162
-909.424292	-2.639878	1.216166
-913.153212	-4.940517	1.221171
-916.746964	-1.230947	1.226176
-920.195210	-10.863510	1.231181
-924.284583	-4.165224	1.236186
-928.203641	-3.057621	1.241190
-931.659861	-6.265998	1.246195
-935.461267	1.822862	1.251200
-938.924512	-0.242674	1.256205
-942.733217	4.537359	1.261210
-946.527039	0.405279	1.266214
-950.321068	-6.916917	1.271219
-954.256721	4.618561	1.276224
-958.226223	-5.837337	1.281229
-962.113017	-14.098727	1.286234
-965.482802	0.019197	1.291238
-968.905935	-16.301966	1.296243
-972.978869	-4.014388	1.301248
-976.920435	-8.179558	1.306253
-980.723136	-7.123591	1.311258
-984.519036	-5.184041	1.316262
-988.215674	-4.141869	1.321267
-991.746502	-0.800216	1.326272
-995.667086	-2.838260	1.331277
-999.364568	-3.702460	1.336282
-1003.095069	5.234599	1.341286
-1007.033165	-6.460980	1.346291
-1010.837232	-6.879188	1.351296
-1014.884429	-10.775087	1.356301
-1018.173773	-8.758802	1.361306
-1021.739259	-3.054034	1.366310
-1025.686633	-3.495029	1.371315
-1029.485793	-11.734048	1.376320
-1033.108981	-6.225038	1.381325
-1036.944780	-7.560639	1.386330
-1041.163630	-2.172387	1.391334
-1044.639070	-4.693126	1.396339
-1048.716468	2.083881	1.401344
-1052.084922	-5.629485	1.406349
-1055.363847	-5.721609	1.411354
-1059.422466	4.925383	1.416358
-1063.200826	-1.508157	1.421363
-1067.496081	-0.150917	1.426368
-1071.085325	6.929668	1.431373
-1074.573684	3.195216	1.436378
-1078.244357	3.074323	1.441382
-1081.676478	3.716364	1.446387
-1086.170895	5.670042	1.451392
-1089.719637	-1.348959	1.456397
-1093.475628	0.040338	1.461402
-1097.424393	6.278037	1.466406
-1101.083402	-10.523997	1.471411
-1104.814562	3.888459	1.476416
-1108.074676	-1.870976	1.481421
-1112.264414	0.861906	1.486426
-1116.148088	4.733272	1.491430
-1119.698141	8.298962	1.496435
-1123.851189	0.034711	1.501440
-1127.120497	-10.621201	1.506445
-1130.879475	-14.045764	1.511450
-1134.867747	-13.443981	1.516454
-1138.358378	1.127158	1.521459
-1142.707028	8.964847	1.526464
-1146.204188	1.967644	1.531469
-1149.743839	-2.849727	1.536474
-1153.477201	-6.182161	1.541478
-1157.102513	-10.479615	1.546483
-1161.060863	-1.412829	1.551488
-1165.143787	2.238183	1.556493
-1169.031479	-8.591538	1.561498
-1172.213791	-7.520982	1.566502
-1175.820392	-11.250547	1.571507
-1180.078777	-0.137742	1.576512
-1183.626871	-7.848970	1.581517
-1187.524587	-0.190587	1.586522
-1191.256336	5.485843	1.591526
-1194.604306	-6.791093	1.596531
-1198.706889	-3.499574	1.601536
-1202.519941	2.440614	1.606541
-1206.513679	-2.392318	1.611546
-1210.357951	2.329174	1.616550
-1213.636051	-3.859309	1.621555
-1217.659044	9.283269	1.626560
-1221.109772	5.916756	1.631565
-1224.918566	-7.019669	1.636570
-1229.053204	-11.101465	1.641574
-1232.661624	-1.082896	1.646579
-1236.601456	-3.084333	1.651584
-1240.332193	6.900210	1.656589
-1243.926304	4.272608	1.661594
-1247.519616	-1.854344	1.666598
-1251.128793	-10.662697	1.671603
-1255.472684	1.895782	1.676608
-1259.072805	-1.970307	1.681613
-1262.538977	-5.881480	1.686618
-1266.458421	6.598057	1.691622
-1269.696760	-8.787105	1.696627
-1273.865169	3.867902	1.701632
-1277.869012	-0.575360	1.706637
-1281.787294	2.309919	1.711642
-1285.482382	3.030616	1.716646
-1289.142722	-8.437667	1.721651
-1292.841234	-13.196267	1.726656
-1296.867580	-3.392990	1.731661
-1299.927245	-3.816326	1.736666
-1303.950453	2.791588	1.741670
-1307.436996	-14.793034	1.746675
-1311.387728	-2.869817	1.751680
-1315.183511	-9.432599	1.756685
-1319.134591	-6.382739	1.761690
-1323.166062	-10.748955	1.766694
-1326.592739	-8.366486	1.771699
-1330.521507	-5.622950	1.776704
-1334.559622	-1.814818	1.781709
-1338.109582	-9.921306	1.786714
-1341.473197	1.278784	1.791718
-1345.372750	-12.691554	1.796723
-1349.576735	2.702102	1.801728
-1352.870530	-8.428935	1.806733
-1356.916631	-1.203841	1.811738
-1360.579157	-5.007738	1.816742
-1363.922758	-9.804112	1.821747
-1368.039818	-4.365349	1.826752
-1372.014799	0.785753	1.831757
-1375.429664	-4.183699	1.836762
-1379.179111	3.717758	1.841766
-1382.734980	1.580990	1.846771
-1386.736677	-2.118106	1.851776
-1390.545991	-10.376952	1.856781
-1394.266072	0.074461	1.861786
-1398.206060	-6.283746	1.866790
-1401.580414	-12.997424	1.871795
-1405.789605	-5.191058	1.876800
-1409.728070	-1.110172	1.881805
-1413.020917	-3.978122	1.886810
-1416.674358	-12.982536	1.891814
-1420.526479	-8.685225	1.896819
-1424.420495	-12.704263	1.901824
-1428.195543	-15.043981	1.906829
-1432.236124	-10.093588	1.911834
-1436.039888	-3.941633	1.916838
-1439.431654	-15.671848	1.921843
-1443.190500	-4.069303	1.926848
-1446.740928	1.699914	1.931853
-1450.566202	-8.899599	1.936858
-1454.916979	-6.052014	1.941862
-1458.309400	-12.359017	1.946867
-1461.995549	-5.178769	1.951872
-1465.834926	5.075817	1.956877
-1469.256200	-4.626425	1.961882
-1473.399676	-3.956631	1.966886
-1476.926388	-6.006456	1.971891
-1480.901676	-0.076118	1.976896
-1484.412428	-2.823916	1.981901
-1488.523174	-7.096718	1.986906
-1492.494990	-0.996607	1.991910
-1495.829907	-9.991973	1.996915
-1500.131699	-3.195574	2.006912
-1500.626331	-5.568467	2.016909
-1498.132746	-5.637773	2.026906
-1495.363373	-6.008610	2.036902
-1493.072974	-8.128013	2.046899
-1491.529494	-4.020414	2.056896
-1489.292024	-8.850295	2.066893
-1487.515759	-7.012611	2.076890
-1485.957239	-12.161661	2.086886
-1483.805126	-13.257854	2.096883
-1481.658949	-12.628878	2.106880
-1480.051079	-6.981050	2.116877
-1478.102538	-12.026760	2.126874
-1476.247330	-7.470119	2.136870
-1474.288800	-6.806351	2.146867
-1472.334160	-11.189872	2.156864
-1470.371556	-8.060428	2.166861
-1468.538812	-12.028110	2.176858
-1466.751499	-11.834290	2.186854
-1464.990484	-13.268895	2.196851
-1462.979214	-3.114577	2.206848
-1460.914318	-5.783633	2.216845
-1459.227535	-9.402673	2.226842
-1457.099204	-10.405032	2.236838
-1455.426009	-17.781379	2.246835
-1453.375780	-9.030668	2.256832
-1451.704659	-9.525602	2.266829
-1449.665000	-16.417464	2.276826
-1447.876756	-11.122180	2.286822
-1445.662849	-9.607169	2.296819
-1443.932060	-8.763225	2.306816
-1442.393408	-14.744333	2.316813
-1440.586524	-13.110463	2.326810
-1438.388335	-14.453992	2.336806
-1436.388116	-13.777919	2.346803
-1434.696210	-10.006679	2.356800
-1433.016936	-5.380778	2.366797
-1430.885875	-7.406714	2.376794
-1429.012732	-4.542384	2.386790
-1427.064356	-11.808036	2.396787
-1425.259468	-15.367013	2.406784
-1423.280040	-10.966006	2.416781
-1421.632671	-9.068158	2.426778
-1419.561699	-8.926033	2.436774
-1417.608064	-1.951929	2.446771
-1416.188504	-7.786061	2.456768
-1414.013582	-4.990561	2.466765
-1411.860183	-9.838489	2.476762
-1410.199766	-10.383786	2.486758
-1408.453033	-12.193432	2.496755
-1406.503358	-8.731860	2.506752
-1404.372254	-6.480390	2.516749
-1402.849698	-14.221011	2.526746
-1400.562306	-10.458237	2.536742
-1398.936910	-11.468447	2.546739
-1397.340627	-8.651347	2.556736
-1395.331103	-8.871995	2.566733
-1393.245850	-10.165822	2.576730
-1391.346977	-13.673504	2.586726
-1389.757524	-13.801634	2.596723
-1387.774911	-10.939006	2.606720
-1385.852474	-9.707276	2.616717
-1383.750183	-2.368517	2.626714
-1382.123576	-4.886812	2.636710
-1379.875415	-5.870390	2.646707
-1378.286763	-5.788383	2.656704
-1376.508585	-8.143043	2.666701
-1374.660398	-7.786790	2.676698
-1372.802445	-7.523678	2.686694
-1370.555210	-10.518687	2.696691
-1368.774567	-10.334776	2.706688
-1367.129545	-8.690724	2.716685
-1364.936678	-6.142786	2.726682
-1363.129628	-12.855237	2.736678
-1361.580185	-10.480615	2.746675
-1359.492303	-10.026930	2.756672
-1357.712590	-11.862345	2.766669
-1355.737569	-15.064818	2.776666
-1353.601574	-16.481996	2.786662
-1351.877443	-12.193216	2.796659
-1350.425042	-5.563556	2.806656
-1348.355845	-4.628446	2.816653
-1346.322874	-12.307054	2.826650
-1344.425052	-10.711347	2.836646
-1342.637566	-11.782201	2.846643
-1340.803768	-8.429918	2.856640
-1338.902633	-10.507388	2.866637
-1336.803911	-11.242791	2.876634
-1335.006825	-13.251497	2.886630
-1332.915740	-7.207218	2.896627
-1331.588013	-14.248714	2.906624
-1329.581205	-9.992531	2.916621
-1327.437027	-7.248868	2.926618
-1325.861061	-6.506369	2.936614
-1323.813143	-6.947839	2.946611
-1321.911417	-11.979616	2.956608
-1320.133013	-11.032673	2.966605
-1318.363071	-7.005409	2.976602
-1316.219075	-3.699597	2.986598
-1314.344257	-4.462301	2.996595
-1312.740315	-1.850049	3.006592
-1310.604073	-6.210403	3.016589
-1308.616843	-6.016879	3.026586
-1306.666379	-12.419085	3.036582
-1304.847057	-14.462905	3.046579
-1303.329793	-8.707284	3.056576
-1301.461277	-9.415285	3.066573
-1299.624218	-2.763468	3.076570
-1297.590637	-7.738963	3.086566
-1295.728973	-10.162188	3.096563
-1293.840436	-4.353874	3.106560
-1292.117909	-8.625892	3.116557
-1289.901279	-9.545915	3.126554
-1288.143618	-14.393555	3.136550
-1286.232606	-13.122018	3.146547
-1284.403181	-4.351587	3.156544
-1282.455527	-7.154882	3.166541
-1280.806415	-8.786178	3.176538
-1278.720760	-7.831534	3.186534
-1276.669637	-7.086099	3.196531
-1275.161517	-4.084272	3.206528
-1273.426866	-1.886071	3.216525
-1271.078803	-4.568701	3.226522
-1269.219294	-4.361018	3.236518
-1267.534100	-1.701736	3.246515
-1265.844403	1.506304	3.256512
-1263.895829	-2.261868	3.266509
-1261.852504	-6.458888	3.276506
-1259.725904	-9.589225	3.286502
-1257.993554	-12.146464	3.296499
-1256.428146	-3.881654	3.306496
-1254.456134	-8.698838	3.316493
-1252.243723	-7.121818	3.326490
-1250.657561	-5.735106	3.336486
-1248.926141	-7.917976	3.346483
-1247.015938	-5.747849	3.356480
-1244.969843	-12.509524	3.366477
-1243.103504	-0.053358	3.376474
-1241.089497	-9.473599	3.386470
-1239.194402	-12.369501	3.396467
-1237.842247	-12.129551	3.406464
-1235.593119	-10.702076	3.416461
-1233.563918	-12.383111	3.426458
-1231.761113	-12.280009	3.436454
-1229.978864	-14.020996	3.446451
-1228.056540	-2.873259	3.456448
-1226.499576	-8.167166	3.466445
-1224.457011	-13.972989	3.476442
-1222.347029	-6.883199	3.486438
-1220.611034	-8.073616	3.496435
-1218.676053	-9.771140	3.506432
-1216.919910	-5.935798	3.516429
-1215.012235	-8.994748	3.526426
-1213.211174	-13.190855	3.536422
-1210.895135	-8.489831	3.546419
-1209.102199	-5.181425	3.556416
-1207.378099	-0.311465	3.566413
-1205.869029	-6.068226	3.576410
-1203.751869	-9.384900	3.586406
-1201.477132	-4.244621	3.596403
-1200.229475	-5.353727	3.606400
-1198.406931	-6.300607	3.616397
-1196.339856	-0.841302	3.626394
-1194.137989	-0.112018	3.636390
-1192.477962	-0.639729	3.646387
-1190.367954	2.322694	3.656384
-1188.799728	-4.654584	3.666381
-1186.774134	-5.859735	3.676378
-1184.961314	-8.912959	3.686374
-1183.073151	2.407660	3.696371
-1181.208519	-4.421249	3.706368
-1179.161629	-4.668214	3.716365
-1177.387401	-2.931012	3.726362
-1175.594724	-4.634153	3.736358
-1173.753137	-8.200396	3.746355
-1171.955089	-2.053810	3.756352
-1169.916132	-9.638500	3.766349
-1167.903589	-5.300979	3.776346
-1166.040630	-3.139014	3.786342
-1164.138217	-4.416017	3.796339
-1162.376450	-3.065232	3.806336
-1160.899480	-4.665747	3.816333
-1158.599416	-2.467918	3.826330
-1156.800861	-9.005180	3.836326
-1154.879560	-5.644636	3.846323
-1153.105136	-6.140095	3.856320
-1151.239391	-6.650162	3.866317
-1149.193865	0.794230	3.876314
-1147.708678	-8.127648	3.886310
-1145.595447	-1.581461	3.896307
-1143.549564	-4.334044	3.906304
-1141.633989	-4.234702	3.916301
-1140.004370	-4.171717	3.926298
-1138.060940	-0.903119	3.936294
-1136.174139	-4.827097	3.946291
-1134.320472	-6.247858	3.956288
-1132.344774	-12.563965	3.966285
-1130.307203	-8.522523	3.976282
-1128.539422	-13.126931	3.986278
-1126.643608	-10.905453	3.996275
-1125.016413	-9.327847	4.006272
-1123.068980	-0.760888	4.016269
-1121.221516	-9.634916	4.026266
-1119.294424	-10.563722	4.036262
-1117.381251	-11.172930	4.046259
-1115.612152	-13.830682	4.056256
-1113.761947	-5.881326	4.066253
-1111.608738	-11.303702	4.076250
-1109.830150	-12.301903	4.086246
-1107.856705	-14.632336	4.096243
-1106.016634	-9.525059	4.106240
-1104.430924	-7.141849	4.116237
-1102.434055	-11.776570	4.126234
-1100.386362	-14.999933	4.136230
-1098.543269	-19.207415	4.146227
-1096.901705	-13.143108	4.156224
-1095.045624	-11.237355	4.166221
-1092.911820	-14.946596	4.176218
-1091.238435	-16.575328	4.186214
-1089.201846	-17.400045	4.196211
-1087.358535	-10.671679	4.206208
-1085.319425	-10.322050	4.216205
-1083.567195	-12.468656	4.226202
-1081.743039	-17.009415	4.236198
-1079.691175	-11.354938	4.246195
-1078.191936	-17.080047	4.256192
-1075.924000	-10.489068	4.266189
-1074.066483	-15.196213	4.276186
-1072.460309	-17.499449	4.286182
-1070.820993	-16.094271	4.296179
-1068.498711	-9.584609	4.306176
-1066.630125	-5.178180	4.316173
-1065.015141	-8.439671	4.326170
-1062.700344	-11.250987	4.336166
-1060.667529	-14.244568	4.346163
-1059.336388	-11.146392	4.356160
-1057.326985	-11.658836	4.366157
-1055.672070	-6.646638	4.376154
-1053.638288	-14.610935	4.386150
-1051.543009	-14.030259	4.396147
-1049.602286	-10.746943	4.406144
-1048.416061	-13.306682	4.416141
-1046.067171	-15.870800	4.426138
-1044.067783	-16.819003	4.436134
-1042.278053	-14.901016	4.446131
-1040.566518	-16.976344	4.456128
-1038.639851	-11.747071	4.466125
-1036.545726	-9.045651	4.476122
-1034.874786	-14.430300	4.486118
-1033.072393	-11.901695	4.496115
-1030.847617	-12.214876	4.506112
-1029.111411	-11.009903	4.516109
-1027.230205	-8.924954	4.526106
-1025.489189	-11.257620	4.536102
-1023.491370	-10.568172	4.546099
-1021.693402	-5.994094	4.556096
-1020.130026	-8.622033	4.566093
-1017.938973	-10.188241	4.576090
-1015.980320	-10.019896	4.586086
-1014.294698	-12.738436	4.596083
-1012.431568	-9.895840	4.606080
-1010.279257	-6.480537	4.616077
-1008.522663	-14.910473	4.626074
-1006.575772	-11.408631	4.636070
-1004.755241	-5.123394	4.646067
-1003.042380	-6.000477	4.656064
-1001.061732	-6.950383	4.666061
-999.170868	-4.170632	4.676058
-997.267399	-4.516082	4.686054
-995.348314	-6.420885	4.696051
-993.785467	-4.086045	4.706048
-991.614587	-2.593711	4.716045
-989.758614	-11.694799	4.726042
-987.917772	-10.083367	4.736038
-986.112548	-3.490926	4.746035
-984.091617	-0.124061	4.756032
-982.397679	-9.906608	4.766029
-980.428859	-8.388268	4.776026
-978.299466	-16.010950	4.786022
-976.633078	-17.030582	4.796019
-975.045379	-11.557571	4.806016
-972.859307	-11.766613	4.816013
-970.987859	-18.163818	4.826010
-969.059345	-17.824823	4.836006
-967.089845	-15.801313	4.846003
-965.273862	-15.261161	4.856000
-963.664314	-19.388564	4.865997
-961.810476	-17.289712	4.875994
-959.755723	-13.102439	4.885990
-957.675705	-17.723496	4.895987
-956.051532	-19.349000	4.905984
-954.056759	-18.539005	4.915981
-952.274753	-10.371759	4.925978
-950.329910	-19.638607	4.935974
-948.792950	-17.708550	4.945971
-946.564349	-15.476977	4.955968
-944.694669	-19.843334	4.965965
-943.052710	-15.067404	4.975962
-941.035542	-8.650924	4.985958
-939.128091	-13.725957	4.995955
-937.259025	-15.772716	5.005952
-935.356698	-11.774208	5.015949
-933.521601	-12.541310	5.025946
-931.514244	-16.781249	5.035942
-929.735114	-18.496250	5.045939
-927.879021	-11.716107	5.055936
-926.062616	-10.977041	5.065933
-924.105055	-13.164257	5.075930
-922.288527	-8.852015	5.085926
-920.063845	-11.023517	5.095923
-918.378060	-10.860408	5.105920
-916.830210	-5.232558	5.115917
-914.869302	-11.053497	5.125914
-912.616772	-12.304171	5.135910
-911.035976	-11.115314	5.145907
-909.241710	-8.356359	5.155904
-907.255191	-14.790866	5.165901
-905.005730	-12.415743	5.175898
-903.473811	-6.935338	5.185894
-901.657255	-12.035285	5.195891
-899.647839	-8.832295	5.205888
-897.786430	-4.542997	5.215885
-896.096872	-9.655795	5.225882
-893.926972	-4.182644	5.235878
-892.199464	-15.206829	5.245875
-890.346256	-13.047816	5.255872
-888.631524	-9.546649	5.265869
-886.647886	-6.228999	5.275866
-884.730487	-9.215034	5.285862
-882.926390	-7.303955	5.295859
-881.092428	2.138750	5.305856
-878.754953	-9.167688	5.315853
-877.074408	2.205358	5.325850
-875.561576	-3.370233	5.335846
-873.368836	-2.538131	5.345843
-871.466196	-12.305027	5.355840
-869.827410	-4.984820	5.365837
-867.682653	-8.589827	5.375834
-865.756868	-4.227109	5.385830
-864.033082	-13.949615	5.395827
-862.446736	-10.454746	5.405824
-860.437565	-3.501641	5.415821
-858.496535	-9.805680	5.425818
-856.451234	-15.790065	5.435814
-854.533369	-16.350862	5.445811
-852.749507	-12.585979	5.455808
-851.252516	-13.360547	5.465805
-849.059493	-6.198400	5.475802
-847.169085	-9.159564	5.485798
-845.180203	-9.141173	5.495795
-843.404746	-12.079221	5.505792
-841.715852	-6.521233	5.515789
-839.558548	-11.252443	5.525786
-838.103003	-10.348254	5.535782
-836.041866	-14.070919	5.545779
-833.897652	-12.323120	5.555776
-832.333541	-7.708346	5.565773
-830.195691	-8.495343	5.575770
-828.443660	-5.079039	5.585766
-826.564382	-7.901038	5.595763
-824.360179	-7.225462	5.605760
-822.723001	-8.834009	5.615757
-821.048134	-4.930096	5.625754
-819.139141	-5.978924	5.635750
-817.255941	-13.312646	5.645747
-815.216811	-10.188543	5.655744
-813.267135	-8.930686	5.665741
-811.780264	1.412307	5.675738
-809.544140	-2.941475	5.685734
-807.643306	-7.326924	5.695731
-806.052729	-4.282694	5.705728
-804.019583	-2.870800	5.715725
-802.350014	-6.527693	5.725722
-800.045544	-12.318194	5.735718
-798.233872	-12.729337	5.745715
-796.508486	-5.107123	5.755712
-794.502235	-0.768256	5.765709
-792.924099	-5.632648	5.775706
-790.901529	-3.841680	5.785702
-789.021132	-8.762275	5.795699
-787.062329	-7.232693	5.805696
-785.383682	-7.129928	5.815693
-783.889608	-7.213980	5.825690
-781.390417	-8.016054	5.835686
-779.505355	-8.748391	5.845683
-777.870372	-3.718584	5.855680
-775.789320	-1.791684	5.865677
-773.834558	-4.886238	5.875674
-772.039148	-10.794301	5.885670
-770.336463	-3.848971	5.895667
-768.409317	-3.034322	5.905664
-766.479261	0.779900	5.915661
-764.635084	0.936751	5.925658
-762.635433	-3.619197	5.935654
-760.730554	-2.043079	5.945651
-759.087879	-5.851962	5.955648
-757.604087	0.278881	5.965645
-755.285011	-0.655435	5.975642
-752.923713	-4.107054	5.985638
-751.610829	-5.358984	5.995635
-749.555211	-2.321140	6.005632
-747.782610	-1.402827	6.015629
-746.099825	-3.114928	6.025626
-743.897445	-4.973226	6.035622
-742.053236	-8.061139	6.045619
-740.178527	-9.432850	6.055616
-738.233854	-0.113505	6.065613
-736.287523	-15.366302	6.075610
-734.554813	-12.677900	6.085606
-733.002977	-12.204301	6.095603
-731.095207	-13.121810	6.105600
-728.763810	-6.218500	6.115597
-726.905656	-9.234418	6.125594
-725.102884	-11.807268	6.135590
-723.547970	-9.687293	6.145587
-721.582722	-7.828682	6.155584
-719.622199	-8.591979	6.165581
-717.665123	-7.772598	6.175578
-715.965517	-7.362076	6.185574
-713.878231	-10.919870	6.195571
-711.710477	-11.072057	6.205568
-710.240748	-6.148425	6.215565
-708.443457	-6.208251	6.225562
-706.619198	-5.329741	6.235558
-704.770945	-5.148231	6.245555
-702.728706	-6.510368	6.255552
-700.796839	-3.959554	6.265549
-698.851767	-6.632494	6.275546
-697.149199	-10.337221	6.285542
-695.139973	-3.262391	6.295539
-693.110264	-2.609334	6.305536
-691.376873	-4.992650	6.315533
-689.520583	-3.148180	6.325530
-687.879175	-7.361030	6.335526
-686.167195	-9.139334	6.345523
-683.681175	-1.880150	6.355520
-681.859465	-6.442337	6.365517
-680.210326	-13.624874	6.375514
-678.545000	-10.901977	6.385510
-676.244711	4.022784	6.395507
-674.630832	-4.913092	6.405504
-672.780774	-1.864438	6.415501
-670.950806	3.407457	6.425498
-669.040905	1.867543	6.435494
-666.647341	-2.643900	6.445491
-665.067611	-6.347926	6.455488
-663.325341	-4.418900	6.465485
-661.402033	-7.672551	6.475482
-659.396881	-14.476164	6.485478
-657.764416	-11.939056	6.495475
-655.749006	-7.168893	6.505472
-654.108410	-10.737371	6.515469
-652.076350	-10.218867	6.525466
-650.463790	-8.103316	6.535462
-647.899579	-6.460344	6.545459
-646.253996	-13.749662	6.555456
-644.693500	-7.599420	6.565453
-642.532447	-10.598932	6.575450
-640.747833	-12.156700	6.585446
-638.973110	-7.292803	6.595443
-637.152142	-11.014827	6.605440
-634.958505	-7.894720	6.615437
-633.277816	-10.367471	6.625434
-631.423437	-10.516886	6.635430
-629.528716	-6.614797	6.645427
-627.475595	-5.472786	6.655424
-626.440963	1.377287	6.665421
-623.986349	-2.272278	6.675418
-621.953690	-5.638107	6.685414
-619.794771	-7.293557	6.695411
-618.205120	-9.192797	6.705408
-616.382715	-6.051259	6.715405
-614.571462	-6.867991	6.725402
-612.461377	-14.242550	6.735398
-610.829133	-10.480094	6.745395
-608.879178	-9.915278	6.755392
-607.159719	-7.933617	6.765389
-605.123987	-13.101526	6.775386
-603.195951	-16.074829	6.785382
-601.250106	-10.339808	6.795379
-599.798508	-4.326873	6.805376
-597.653317	-7.983822	6.815373
-595.599444	-8.452452	6.825370
-594.049547	-6.221058	6.835366
-591.912786	-15.404624	6.845363
-590.139229	-11.454725	6.855360
-588.366782	-11.933655	6.865357
-586.424488	-14.006053	6.875354
-584.642812	-12.410110	6.885350
-582.524383	-12.026924	6.895347
-580.517598	-13.326451	6.905344
-579.121948	-3.338195	6.915341
-577.046060	-4.754550	6.925338
-575.007480	-9.839205	6.935334
-573.191359	-12.245126	6.945331
-571.447709	-9.319922	6.955328
-569.631415	-8.225294	6.965325
-567.498915	-12.808622	6.975322
-565.729916	-17.434935	6.985318
-564.140957	-8.683883	6.995315
-561.425457	-9.905549	7.005312
-559.825266	-9.486930	7.015309
-558.630814	-9.107709	7.025306
-556.599123	-15.618635	7.035302
-554.266993	-8.778417	7.045299
-552.437967	-13.085885	7.055296
-550.997847	-12.224843	7.065293
-548.777932	-12.293633	7.075290
-546.854326	-13.447213	7.085286
-545.226286	-11.910384	7.095283
-543.317798	-13.445235	7.105280
-541.222836	-10.926655	7.115277
-539.441360	-11.784365	7.125274
-537.781315	-9.406315	7.135270
-535.734181	-12.998598	7.145267
-534.244744	-15.248098	7.155264
-531.742325	-6.308183	7.165261
-529.948388	-8.631581	7.175258
-528.181194	-9.757005	7.185254
-526.281123	-9.231521	7.195251
-524.624561	-8.705038	7.205248
-522.498988	-9.063476	7.215245
-520.597826	-5.146534	7.225242
-519.105942	-10.843309	7.235238
-516.927821	-7.043233	7.245235
-515.130788	-2.680173	7.255232
-513.197246	-3.378991	7.265229
-511.350114	-12.112019	7.275226
-509.427918	-9.066861	7.285222
-507.437888	-10.347862	7.295219
-505.855347	-3.098917	7.305216
-503.759842	-6.646795	7.315213
-501.997500	-3.576099	7.325210
-499.880019	-4.651657	7.335206
-498.108856	-17.329440	7.345203
-496.396893	-7.934814	7.355200
-494.387277	-7.835754	7.365197
-492.549843	-10.087123	7.375194
-490.558797	-6.367672	7.385190
-488.800903	-12.283758	7.395187
-487.020736	-8.849577	7.405184
-485.231646	-4.134694	7.415181
-483.261770	1.069222	7.425178
-481.242585	-4.413322	7.435174
-479.333948	-4.763918	7.445171
-477.484093	-8.289911	7.455168
-475.464339	-5.885577	7.465165
-473.812539	-7.014638	7.475162
-472.029703	0.066555	7.485158
-469.844889	-6.320339	7.495155
-468.009597	-10.958752	7.505152
-466.396149	-15.362785	7.515149
-464.571242	-9.115689	7.525146
-462.764381	-11.172677	7.535142
-460.618002	-7.083263	7.545139
-458.614544	-6.668974	7.555136
-457.045694	-9.779018	7.565133
-455.018472	-7.139013	7.575130
-453.048924	-14.288893	7.585126
-451.199822	-5.037709	7.595123
-449.238064	-5.219920	7.605120
-447.680687	-4.314380	7.615117
-445.693035	-1.806996	7.625114
-443.796678	-6.153562	7.635110
-441.826657	-1.458062	7.645107
-439.758121	-5.674222	7.655104
-438.364143	0.510659	7.665101
-436.144491	-1.196958	7.675098
-434.587067	-7.513636	7.685094
-432.720910	-10.170606	7.695091
-430.671095	-6.730491	7.705088
-428.515514	-4.710969	7.715085
-426.767081	1.268896	7.725082
-424.894433	-6.130761	7.735078
-423.152603	0.079112	7.745075
-421.386149	-6.365676	7.755072
-419.292149	-1.903115	7.765069
-417.728292	-1.661757	7.775066
-415.658507	-3.506480	7.785062
-413.616234	-4.238370	7.795059
-411.557415	-7.835576	7.805056
-410.477701	-6.375311	7.815053
-408.505875	-1.196905	7.825050
-406.149410	1.079515	7.835046
-404.069167	-6.485909	7.845043
-402.394348	-4.201700	7.855040
-400.634775	0.200592	7.865037
-398.646607	1.771603	7.875034
-396.906540	6.255963	7.885030
-395.144363	-1.795522	7.895027
-393.101625	-2.751682	7.905024
-391.028011	-2.424328	7.915021
-389.442773	1.634750	7.925018
-387.367860	1.312941	7.935014
-385.472228	-3.128204	7.945011
-384.128320	-3.933304	7.955008
-382.051223	-4.975468	7.965005
-379.827578	4.710203	7.975002
-378.224048	-2.734877	7.984998
-376.140421	-8.605001	7.994995
-374.159163	-4.623354	8.004992
-372.589392	-1.449178	8.014989
-370.627783	-3.327119	8.024986
-368.703224	-0.743279	8.034982
-366.891458	-3.317305	8.044979
-365.109934	-4.364371	8.054976
-362.950546	-1.562225	8.064973
-361.060161	3.709756	8.074970
-359.199931	-1.938371	8.084966
-357.249790	0.314547	8.094963
-355.970432	0.454522	8.104960
-353.926493	-0.171792	8.114957
-351.756919	-0.210257	8.124954
-349.717663	-4.726411	8.134950
-348.065979	0.403685	8.144947
-346.131339	-1.937307	8.154944
-344.329102	1.774522	8.164941
-342.612271	-5.483358	8.174938
-340.595709	-1.267313	8.184934
-338.570516	-0.227960	8.194931
-336.668449	0.189986	8.204928
-334.950565	-4.818018	8.214925
-333.124101	-4.324840	8.224922
-331.145624	2.384179	8.234918
-329.376775	-2.131423	8.244915
-327.821883	-2.706485	8.254912
-325.487315	0.438790	8.264909
-323.496869	-4.653772	8.274906
-321.916178	0.133986	8.284902
-319.885941	-8.498670	8.294899
-318.021366	1.088066	8.304896
-316.174539	0.647990	8.314893
-314.475908	-3.120590	8.324890
-312.392167	-0.251056	8.334886
-310.357142	2.561519	8.344883
-308.516439	-1.989225	8.354880
-306.763017	-2.387540	8.364877
-305.201665	-1.258325	8.374874
-303.227378	-3.583507	8.384870
-301.253545	-5.174392	8.394867
-299.166813	0.871574	8.404864
-297.138029	3.591998	8.414861
-295.650641	-1.323924	8.424858
-293.657768	-2.022563	8.434854
-291.572644	0.480447	8.444851
-289.949793	2.343553	8.454848
-288.217501	-6.326785	8.464845
-286.197558	-2.280182	8.474842
-284.367647	1.403593	8.484838
-282.179101	0.225300	8.494835
-280.420146	-5.562922	8.504832
-278.719423	1.746279	8.514829
-276.771307	2.704828	8.524826
-274.957950	-10.230621	8.534822
-273.316868	-3.641385	8.544819
-271.051443	-5.187208	8.554816
-269.180900	0.100648	8.564813
-267.368960	-1.906482	8.574810
-265.590560	0.113394	8.584807
-263.658124	-3.223515	8.594803
-261.693900	-6.617603	8.604800
-259.968001	-1.347706	8.614797
-257.931179	-3.734940	8.624794
-256.335248	0.101468	8.634791
-254.186527	-4.124181	8.644787
-252.323119	-1.224163	8.654784
-250.384666	1.404927	8.664781
-248.700353	-0.348130	8.674778
-246.896785	-1.570736	8.684775
-245.071923	0.724377	8.694771
-242.956794	-4.099071	8.704768
-240.986978	-1.942356	8.714765
-239.301627	-0.157087	8.724762
-237.430704	-9.558478	8.734759
-235.403249	-4.624066	8.744755
-233.660155	-7.630727	8.754752
-231.801085	-1.418888	8.764749
-229.722716	-0.766884	8.774746
-228.117825	1.103868	8.784743
-225.938012	-2.695660	8.794739
-224.048879	-3.654006	8.804736
-222.369885	-4.237754	8.814733
-220.243246	-13.626257	8.824730
-218.652003	-10.629092	8.834727
-216.767202	-14.728901	8.844723
-214.610826	-14.790399	8.854720
-213.065808	-14.392742	8.864717
-211.109145	-15.060270	8.874714
-209.290742	-10.864593	8.884711
-207.333558	-15.935963	8.894707
-205.340084	-16.768838	8.904704
-203.794528	-8.392697	8.914701
-201.864117	-7.300207	8.924698
-199.910970	-11.022484	8.934695
-197.941187	-12.781589	8.944691
-196.009155	-12.783583	8.954688
-194.250522	-11.425249	8.964685
-192.356698	-12.643270	8.974682
-190.785222	-7.550787	8.984679
-188.586808	-11.479568	8.994675
-186.581655	-9.851089	9.004672
-185.054062	-9.687478	9.014669
-182.977093	-14.438467	9.024666
-181.161087	-17.125140	9.034663
-179.344184	-11.268118	9.044659
-177.368523	-15.305027	9.054656
-175.491435	-20.399907	9.064653
-173.334694	-5.202202	9.074650
-171.747881	-11.907108	9.084647
-169.724972	-10.898828	9.094643
-167.964474	-18.005661	9.104640
-166.190020	-15.389808	9.114637
-164.170845	-11.063499	9.124634
-162.676397	-10.856690	9.134631
-160.330910	-16.149465	9.144627
-158.584765	-16.121767	9.154624
-156.779554	-13.049753	9.164621
-154.862414	-11.784578	9.174618
-152.930020	-7.689152	9.184615
-151.022678	-3.828150	9.194611
-149.183090	-7.049101	9.204608
-147.316787	-11.235910	9.214605
-145.226965	-9.901964	9.224602
-143.544335	-13.255762	9.234599
-141.655606	-15.529267	9.244595
-139.904225	-16.898206	9.254592
-137.784268	-15.403270	9.264589
-136.308549	-17.212967	9.274586
-134.479671	-17.468458	9.284583
-132.190340	-15.875804	9.294579
-130.230144	-16.395407	9.304576
-128.496982	-13.371876	9.314573
-126.979448	-11.763439	9.324570
-124.870404	-10.694653	9.334567
-123.001805	-14.144427	9.344563
-120.982044	-9.712381	9.354560
-119.139929	-5.030930	9.364557
-117.118919	-8.571337	9.374554
-115.618201	-9.663418	9.384551
-113.496569	-10.121922	9.394547
-111.583039	-7.379792	9.404544
-109.854959	-9.861330	9.414541
-108.103933	-2.656341	9.424538
-106.140567	-1.273762	9.434535
-104.029162	-4.517523	9.444531
-102.188647	1.710019	9.454528
-100.407674	-0.522579	9.464525
-98.340945	2.365651	9.474522
-96.828777	-2.183052	9.484519
-94.959163	-6.577199	9.494515
-92.785689	-1.174893	9.504512
-91.154945	3.513464	9.514509
-89.018453	-4.062268	9.524506
-87.347081	-0.392517	9.534503
-85.516106	-1.575167	9.544499
-83.501303	-7.282494	9.554496
-81.811775	4.771901	9.564493
-79.878369	-3.399858	9.574490
-78.077801	-2.785510	9.584487
-75.913945	-3.375457	9.594483
-74.270861	1.441998	9.604480
-72.276301	-0.488332	9.614477
-70.299363	-5.295908	9.624474
-68.550092	-3.283867	9.634471
-66.456096	-6.403237	9.644467
-64.932302	0.365925	9.654464
-62.850521	-3.908886	9.664461
-61.005891	-0.587289	9.674458
-58.977632	1.031298	9.684455
-57.353651	-10.561675	9.694451
-55.217138	-5.009751	9.704448
-53.746053	-5.822326	9.714445
-51.602052	-4.122722	9.724442
-49.845355	-0.648138	9.734439
-48.109812	-9.525690	9.744435
-45.788188	-7.710730	9.754432
-43.949191	-7.841449	9.764429
-42.179289	-2.002076	9.774426
-40.459553	-2.825887	9.784423
-38.839442	-0.809010	9.794419
-36.562135	-1.971241	9.804416
-34.875282	0.222890	9.814413
-32.703473	-5.185754	9.824410
-31.017739	-8.628397	9.834407
-29.032465	-0.451743	9.844403
-27.279412	-2.117718	9.854400
-25.526939	2.068100	9.864397
-23.389391	3.118220	9.874394
-21.499126	-3.851328	9.884391
-19.924927	1.405058	9.894387
-17.849173	-1.322934	9.904384
-16.112475	-0.210446	9.914381
-14.012373	-1.464393	9.924378
-12.111786	0.821981	9.934375
-10.630671	-4.591737	9.944371
-8.123823	-2.141534	9.954368
-6.601805	-0.315834	9.964365
-4.991084	4.200513	9.974362
-3.421435	21.584222	9.984359
-2.075019	49.999616	9.994355
-0.652676	100.459869	10.004352
0.000000	140.861295	10.009357
0.992430	159.095292	10.014362
1.720921	189.995148	10.019367
2.298267	222.983453	10.024371
2.607435	245.453516	10.029376
2.791112	257.035592	10.034381
3.322800	266.713935	10.039386
3.141862	284.392488	10.044391
3.371055	284.977271	10.049395
3.505238	297.552894	10.054400
3.499275	295.544762	10.059405
3.548090	296.871118	10.064410
3.493037	305.108660	10.069415
3.697162	296.811081	10.074419
3.721894	301.326807	10.079424
3.760171	313.685923	10.084429
4.136181	313.816770	10.089434
4.015725	321.252600	10.094439
4.290789	328.803548	10.099443
3.796048	323.683109	10.104448
4.134501	335.087591	10.109453
4.348404	346.508795	10.114458
4.337027	352.701915	10.119463
4.651676	342.208845	10.124467
4.468815	323.332972	10.129472
4.244560	322.775797	10.134477
4.542084	323.430110	10.139482
4.343312	326.194756	10.144487
4.280398	322.910451	10.149491
4.792540	337.546883	10.154496
4.763274	332.612400	10.159501
4.806817	324.660550	10.164506
4.646220	328.783209	10.169511
4.505471	329.966335	10.174515
4.604286	328.299464	10.179520
4.697127	349.252429	10.184525
5.408033	345.163427	10.189530
5.014255	342.460187	10.194535
4.838368	340.149559	10.199539
4.674239	342.224265	10.204544
4.692233	354.481781	10.209549
5.388912	359.615766	10.214554
5.045039	375.032190	10.219559
5.183714	373.404689	10.224563
5.326917	369.850946	10.229568
5.001914	376.409501	10.234573
5.461373	378.373709	10.239578
5.363546	378.654255	10.244583
5.391969	384.978240	10.249587
5.448673	386.684980	10.254592
5.416757	386.999170	10.259597
6.052094	380.249192	10.264602
5.267277	381.732179	10.269607
5.472097	379.785034	10.274611
5.565274	385.430041	10.279616
5.642098	389.951678	10.284621
5.961380	387.243507	10.289626
5.757698	392.511653	10.294631
5.791219	399.744762	10.299635
5.742398	403.472710	10.304640
5.693898	409.181327	10.309645
5.542325	399.628356	10.314650
5.629206	407.412795	10.319655
5.708470	399.603444	10.324659
5.895833	399.441096	10.329664
5.823950	399.878359	10.334669
5.891212	401.622843	10.339674
6.078720	420.972768	10.344679
6.205326	429.001626	10.349683
6.409205	428.481817	10.354688
6.326865	436.129253	10.359693
6.728084	432.610038	10.364698
6.489950	441.976034	10.369703
6.477140	430.607850	10.374707
6.552864	439.264594	10.379712
6.218665	444.950983	10.384717
6.293310	440.441452	10.389722
6.308646	450.561838	10.394727
6.453060	448.875063	10.399731
6.446617	437.726640	10.404736
6.450830	454.833376	10.409741
6.720761	439.335630	10.414746
6.385303	453.096512	10.419751
6.519304	467.186241	10.424755
6.674979	468.170704	10.429760
6.467433	478.058567	10.434765
7.039032	486.488006	10.439770
7.012898	482.975439	10.444775
7.091745	489.365546	10.449779
6.792251	480.700320	10.454784
6.775166	485.676953	10.459789
6.981907	480.823051	10.464794
7.101306	504.705250	10.469799
7.088618	509.186006	10.474803
7.603708	502.105055	10.479808
7.454288	506.554001	10.484813
7.690989	510.575494	10.489818
7.510419	507.953336	10.494823
7.618564	514.354551	10.499827
7.836055	516.649121	10.504832
7.593802	527.318445	10.509837
8.004667	514.124243	10.514842
7.783920	525.509256	10.519847
7.588683	514.277342	10.524851
7.731793	529.368662	10.529856
7.570951	525.223108	10.534861
7.957924	528.493631	10.539866
7.650585	535.412154	10.544871
7.841586	528.509045	10.549875
8.191600	522.411665	10.554880
7.705675	532.279309	10.559885
7.872800	531.949870	10.564890
7.828134	536.782680	10.569895
7.790339	529.969683	10.574899
7.984759	547.486178	10.579904
8.344298	554.091751	10.584909
8.345807	550.628377	10.589914
8.355355	564.585081	10.594919
8.681568	561.252848	10.599923
8.379457	567.646981	10.604928
8.321597	570.269343	10.609933
8.435657	568.942227	10.614938
8.635517	575.751482	10.619943
8.426994	573.546951	10.624947
8.787074	576.869086	10.629952
8.357697	575.054612	10.634957
8.627298	569.928869	10.639962
8.146303	578.489982	10.644967
8.752764	584.677698	10.649971
8.960924	598.645335	10.654976
9.197892	609.665657	10.659981
9.367813	601.403325	10.664986
9.162054	588.843598	10.669991
9.127952	582.602447	10.674995
9.097862	581.381904	10.680000
8.904942	577.736638	10.685005
9.056301	588.964573	10.690010
9.018293	602.208197	10.695015
9.193697	614.004777	10.700019
9.538664	615.561483	10.705024
9.182398	616.436791	10.710029
9.429343	609.874822	10.715034
9.437829	611.873145	10.720039
9.174494	617.482063	10.725043
9.549945	612.317343	10.730048
9.218256	616.656617	10.735053
9.634808	617.052251	10.740058
9.584292	624.579587	10.745063
9.699506	623.972984	10.750067
10.096555	619.386741	10.755072
9.505977	628.704989	10.760077
9.747453	614.395945	10.765082
9.794725	627.930357	10.770087
10.021139	645.077573	10.775091
10.236283	654.633194	10.780096
10.049874	643.585861	10.785101
9.938132	627.943779	10.790106
10.108206	646.585545	10.795111
10.326394	657.697213	10.800115
10.574988	649.871759	10.805120
10.242898	644.947622	10.810125
10.083310	632.730593	10.815130
10.499652	653.182944	10.820135
10.246120	656.268638	10.825139
10.771202	653.801997	10.830144
10.703695	651.305289	10.835149
10.699939	641.018917	10.840154
10.174786	643.706365	10.845159
10.350496	648.876240	10.850163
10.618474	647.448869	10.855168
10.428317	666.747391	10.860173
10.830442	654.473867	10.865178
10.538678	661.218068	10.870183
10.512240	665.563864	10.875187
10.736948	666.797540	10.880192
10.715580	668.395336	10.885197
10.654502	651.223309	10.890202
10.386458	659.029800	10.895207
10.967039	677.311224	10.900211
11.458028	672.235293	10.905216
10.850057	683.229583	10.910221
11.007480	677.874101	10.915226
11.096719	678.391334	10.920231
10.844294	682.263797	10.925235
11.398594	684.865814	10.930240
11.295311	687.239962	10.935245
11.369657	679.488020	10.940250
11.027236	682.813413	10.945255
11.203200	685.131982	10.950259
11.329696	700.735512	10.955264
11.704732	714.709762	10.960269
11.860125	714.897883	10.965274
11.990239	716.386362	10.970279
11.753409	707.728352	10.975283
11.865226	692.536269	10.980288
11.622616	695.104539	10.985293
11.632235	697.853363	10.990298
11.955736	719.609055	10.995303
12.049268	722.256185	11.000307
12.144485	718.650085	11.005312
11.940272	728.408268	11.010317
12.126862	722.029349	11.015322
12.219375	727.453810	11.020327
12.253189	721.913013	11.025331
12.411444	721.465130	11.030336
12.393751	721.195130	11.035341
11.961612	709.980348	11.040346
12.167700	718.460339	11.045351
11.979287	717.846965	11.050355
12.243457	716.027512	11.055360
11.846374	725.701333	11.060365
12.278423	732.230763	11.065370
12.157895	729.898626	11.070375
12.241190	740.654960	11.075379
12.625250	742.194406	11.080384
12.897256	760.574042	11.085389
13.048392	752.412397	11.090394
12.826999	743.797637	11.095399
12.549767	738.382143	11.100403
12.837798	747.281190	11.105408
12.798360	750.356411	11.110413
13.060987	753.345604	11.115418
13.225774	755.336365	11.120423
13.381394	749.015994	11.125427
13.088917	735.864386	11.130432
12.664145	746.785345	11.135437
13.210838	746.124110	11.140442
13.350671	750.156389	11.145447
13.235603	756.815676	11.150451
13.376426	749.480472	11.155456
13.471315	764.874636	11.160461
13.644431	749.313151	11.165466
13.226865	759.179505	11.170471
13.487176	758.278503	11.175475
13.588422	756.639582	11.180480
13.349744	761.878748	11.185485
13.834045	759.549488	11.190490
13.689991	754.623708	11.195495
13.603222	762.808217	11.200499
13.897953	762.792755	11.205504
13.576993	768.127053	11.210509
13.669241	756.686660	11.215514
13.543107	757.913223	11.220519
13.613097	757.995111	11.225523
13.698234	762.263212	11.230528
13.388553	770.243569	11.235533
13.845153	770.416766	11.240538
13.978149	786.043008	11.245543
13.619182	797.160101	11.250547
14.400730	794.650954	11.255552
14.064290	795.068920	11.260557
14.297022	785.386585	11.265562
14.281688	791.408625	11.270567
14.492458	784.167909	11.275571
14.524309	791.469293	11.280576
14.578879	800.115433	11.285581
14.611409	786.651727	11.290586
15.005504	790.264971	11.295591
14.503522	794.820703	11.300595
14.509895	795.087791	11.305600
14.670015	806.620445	11.310605
14.504516	793.483226	11.315610
14.698517	799.317330	11.320615
14.978174	799.942976	11.325619
14.957756	787.766701	11.330624
15.084945	789.990558	11.335629
15.227622	777.382976	11.340634
15.233606	786.874269	11.345639
15.177230	788.476084	11.350643
15.027681	784.473743	11.355648
14.855206	786.840019	11.360653
15.110228	789.022985	11.365658
15.328660	796.076979	11.370663
15.356225	788.903331	11.375667
15.484599	783.166067	11.380672
15.527967	796.452086	11.385677
15.462085	792.723420	11.390682
15.560642	787.760509	11.395687
15.354763	782.767305	11.400691
15.389876	767.857053	11.405696
15.198325	786.791659	11.410701
15.662166	794.505141	11.415706
15.640261	793.215462	11.420711
15.539977	798.440452	11.425715
15.574788	786.455654	11.430720
15.439898	788.610919	11.435725
15.566122	786.130599	11.440730
15.864055	796.070525	11.445735
15.692283	792.437601	11.450739
15.763454	784.564676	11.455744
15.488897	794.823008	11.460749
15.921583	793.005055	11.465754
15.795479	806.516821	11.470759
15.920274	822.235879	11.475763
16.180767	818.600239	11.480768
16.194008	815.861951	11.485773
16.300895	819.246605	11.490778
16.340317	823.711262	11.495783
16.068456	817.548936	11.500787
16.430714	818.834809	11.505792
16.426747	822.435854	11.510797
16.686805	820.692743	11.515802
16.577460	824.845216	11.520807
16.503140	820.332518	11.525811
16.727374	824.766120	11.530816
16.460293	826.160258	11.535821
16.461684	824.108299	11.540826
16.655371	815.621268	11.545831
16.780808	834.070109	11.550835
16.748669	821.151307	11.555840
16.558935	822.528377	11.560845
16.922716	823.976443	11.565850
16.785284	821.345770	11.570855
16.486402	825.287186	11.575859
17.114614	831.879998	11.580864
17.296354	842.727946	11.585869
17.035507	826.041767	11.590874
16.910770	836.246267	11.595879
17.061502	845.973148	11.600883
17.136562	855.644292	11.605888
17.161005	851.969018	11.610893
17.357996	853.278100	11.615898
17.102135	856.171806	11.620903
17.050016	857.490657	11.625907
17.406214	843.293986	11.630912
17.303058	852.868966	11.635917
17.550706	861.298255	11.640922
17.483902	850.331041	11.645927
17.328744	851.122243	11.650931
17.651743	842.825896	11.655936
17.250431	863.815840	11.660941
18.150543	872.880707	11.665946
18.277679	869.021881	11.670951
17.731236	865.685256	11.675955
17.935962	846.641219	11.680960
17.712651	861.887530	11.685965
17.669623	872.867551	11.690970
17.993466	883.027346	11.695975
18.214421	878.864952	11.700979
18.334344	878.535150	11.705984
18.001281	877.522189	11.710989
18.233277	872.665707	11.715994
18.514480	879.594605	11.720999
18.521264	881.706786	11.726003
18.498064	876.211295	11.731008
18.593292	879.995242	11.736013
18.457282	876.443331	11.741018
18.597862	871.951537	11.746023
18.730511	873.308732	11.751027
18.508983	856.248793	11.756032
18.498426	864.899051	11.761037
18.847951	870.687876	11.766042
18.582755	869.219361	11.771047
18.443465	875.570310	11.776051
18.650158	878.216767	11.781056
18.815683	882.800110	11.786061
18.734000	882.040386	11.791066
18.812989	884.527429	11.796071
18.715345	883.282940	11.801075
18.810720	873.277080	11.806080
18.843950	880.956782	11.811085
18.927689	875.013699	11.816090
18.927871	878.494240	11.821095
18.825721	884.075973	11.826099
19.129140	893.116168	11.831104
19.236413	903.321560	11.836109
19.650302	912.733681	11.841114
19.487907	907.219377	11.846119
19.326651	908.612413	11.851123
19.587144	900.053173	11.856128
19.528763	900.989801	11.861133
19.378632	895.394692	11.866138
19.552549	902.066305	11.871143
19.271308	908.872023	11.876147
19.357991	913.270818	11.881152
19.444898	917.328933	11.886157
19.650719	915.132383	11.891162
19.475600	911.627705	11.896167
19.598423	919.241095	11.901171
19.753493	908.831423	11.906176
19.665213	914.365221	11.911181
19.397044	912.465060	11.916186
19.957704	922.754281	11.921191
19.774116	939.481505	11.926195
19.993535	940.118344	11.931200
20.224984	947.197146	11.936205
20.190417	945.355923	11.941210
20.434106	938.822713	11.946215
19.949040	942.386973	11.951219
20.471923	943.309747	11.956224
20.261347	944.188646	11.961229
20.265782	938.758114	11.966234
20.619542	945.536690	11.971239
20.318122	940.976592	11.976243
20.623926	934.073906	11.981248
20.421680	944.532135	11.986253
20.521157	946.815634	11.991258
20.314089	946.079060	11.996263
20.249234	956.824489	12.001267
20.614932	965.250780	12.006272
20.747545	970.366140	12.011277
20.946491	972.422451	12.016282
21.088828	977.607230	12.021287
21.130502	957.691703	12.026291
21.122020	942.229945	12.031296
21.213426	951.808653	12.036301
21.417643	938.478283	12.041306
21.048404	941.692886	12.046311
20.908185	940.813176	12.051315
21.216645	933.588346	12.056320
20.953782	945.846211	12.061325
20.853782	924.732678	12.066330
21.301398	913.888385	12.071335
20.703428	920.763551	12.076339
20.818988	911.013083	12.081344
20.569705	907.630629	12.086349
20.714404	905.535299	12.091354
20.409798	920.603813	12.096359
20.352292	931.314933	12.101363
21.088180	938.841590	12.106368
20.697328	948.902521	12.111373
20.770730	946.288663	12.116378
20.931995	944.996566	12.121383
20.847462	937.451189	12.126387
20.698864	929.531231	12.131392
20.645717	926.238923	12.136397
20.842056	937.177660	12.141402
21.171656	936.159933	12.146407
20.811059	931.216587	12.151411
20.625790	917.185061	12.156416
20.281422	920.957126	12.161421
20.882824	939.828539	12.166426
21.438137	934.792727	12.171431
21.104993	920.322703	12.176435
20.935545	910.690239	12.181440
20.857556	916.665550	12.186445
20.935580	910.750173	12.191450
21.033698	913.858686	12.196455
20.775188	910.887738	12.201459
21.037490	899.592010	12.206464
20.568875	912.762663	12.211469
21.001200	915.218588	12.216474
21.139159	912.234871	12.221479
21.132699	907.277630	12.226483
21.212805	901.906010	12.231488
20.997776	915.697008	12.236493
21.076398	894.072448	12.241498
20.738812	891.268669	12.246503
20.627649	882.134739	12.251507
20.934693	888.155867	12.256512
20.651755	891.361425	12.261517
20.768371	883.711449	12.266522
20.738815	879.210516	12.271527
20.501474	884.870586	12.276531
20.730633	896.654092	12.281536
20.804267	910.957323	12.286541
21.004826	909.335664	12.291546
20.856871	897.974476	12.296551
20.730690	896.792888	12.301555
20.984520	885.998449	12.306560
20.865186	889.244149	12.311565
20.428852	897.911871	12.316570
20.853666	883.376190	12.321575
20.416896	893.936448	12.326579
20.756385	898.903661	12.331584
20.575250	919.312905	12.336589
21.069892	922.325057	12.341594
21.050299	926.165179	12.346599
20.739113	919.130658	12.351603
20.790530	899.256237	12.356608
20.650260	907.086637	12.361613
20.717930	910.690472	12.366618
20.813285	916.753260	12.371623
20.913643	920.167367	12.376627
21.084710	907.725467	12.381632
20.683959	894.546826	12.386637
20.889627	896.285065	12.391642
20.974345	898.728616	12.396647
20.868537	897.515392	12.401651
20.713833	890.213060	12.406656
20.787779	900.343335	12.411661
20.674648	894.190354	12.416666
20.650906	898.149410	12.421671
20.740063	892.632838	12.426675
21.061501	894.114476	12.431680
20.759908	903.382072	12.436685
20.911130	896.338469	12.441690
21.080400	896.484953	12.446695
20.794964	902.241016	12.451699
20.969129	894.971388	12.456704
20.701449	900.961177	12.461709
20.811220	901.216506	12.466714
21.019464	895.351334	12.471719
20.774112	900.813979	12.476723
21.269901	897.154984	12.481728
21.107716	899.953327	12.486733
20.922789	896.503836	12.491738
20.997874	895.040973	12.496743
20.521928	903.286056	12.501747
20.638516	899.378439	12.506752
20.687890	902.333864	12.511757
20.742177	905.245925	12.516762
20.713268	902.232050	12.521767
20.936455	894.694389	12.526771
20.865859	893.169600	12.531776
21.098375	903.567919	12.536781
20.834140	906.803616	12.541786
21.130021	895.202894	12.546791
20.705359	889.883401	12.551795
20.648894	894.084234	12.556800
20.709846	896.766557	12.561805
20.993407	886.561927	12.566810
20.765067	883.518359	12.571815
20.792727	876.202717	12.576819
20.629373	869.671378	12.581824
20.353024	882.629977	12.586829
20.652873	900.784563	12.591834
20.919992	904.391280	12.596839
20.618114	902.990117	12.601843
20.940836	897.592419	12.606848
20.866809	903.732684	12.611853
20.911826	903.421137	12.616858
21.131394	902.600747	12.621863
20.876341	899.326455	12.626867
21.006480	885.989024	12.631872
20.857915	879.251881	12.636877
20.586261	875.227986	12.641882
20.541507	880.187088	12.646887
20.481843	889.234727	12.651891
20.788377	898.495217	12.656896
20.802350	900.816002	12.661901
20.743245	902.850379	12.666906
21.326278	905.151369	12.671911
20.849080	898.023481	12.676915
21.098141	878.418782	12.681920
20.729002	880.250277	12.686925
20.686621	879.146795	12.691930
20.919738	878.765820	12.696935
20.835285	879.734993	12.701939
21.001791	875.436195	12.706944
20.699877	882.723046	12.711949
20.717939	880.081755	12.716954
20.801468	878.158622	12.721959
20.885015	886.076323	12.726963
21.093007	874.426553	12.731968
20.875028	879.118374	12.736973
20.712000	886.895619	12.741978
21.053343	880.419405	12.746983
20.749611	878.125925	12.751987
20.990025	880.257616	12.756992
20.544805	878.951863	12.761997
20.694041	882.317162	12.767002
21.050783	875.945733	12.772007
20.486362	883.796459	12.777011
20.911468	878.685233	12.782016
20.674065	885.673195	12.787021
20.678108	880.837299	12.792026
20.625561	879.101461	12.797031
20.495553	880.019548	12.802035
20.796230	880.884713	12.807040
20.531505	884.864854	12.812045
20.601610	884.779556	12.817050
20.569953	889.629333	12.822055
20.616765	893.999786	12.827059
20.736254	895.565678	12.832064
20.961582	910.686862	12.837069
21.018030	904.156722	12.842074
20.988922	898.977577	12.847079
20.836484	894.409501	12.852083
20.930148	885.764907	12.857088
20.583834	888.783440	12.862093
20.816753	886.235620	12.867098
20.651066	885.706929	12.872103
20.392174	895.650575	12.877107
21.027568	895.090313	12.882112
21.153495	886.901073	12.887117
20.729177	883.527617	12.892122
20.904473	875.778393	12.897127
20.688152	881.659051	12.902131
20.839235	878.525003	12.907136
20.662904	883.022513	12.912141
20.809755	880.133584	12.917146
20.852346	883.498545	12.922151
20.489927	892.417843	12.927155
21.075648	889.411602	12.932160
21.040519	885.953992	12.937165
20.882027	886.857698	12.942170
20.777052	884.382696	12.947175
20.805594	891.766666	12.952179
20.876515	886.743470	12.957184
20.618511	895.341744	12.962189
20.900784	893.256015	12.967194
21.042341	890.989289	12.972199
20.898156	893.650710	12.977203
20.952497	886.613101	12.982208
21.090442	887.351247	12.987213
20.465580	895.503376	12.992218
21.148939	888.874829	12.997223
21.022756	895.097531	13.002227
21.053302	889.577692	13.007232
20.867230	897.730804	13.012237
20.945376	892.862582	13.017242
20.923099	885.968090	13.022247
20.612645	880.292895	13.027251
20.657885	877.177306	13.032256
20.748746	887.580860	13.037261
20.587062	898.254951	13.042266
20.627666	895.996441	13.047271
20.678878	898.633007	13.052275
20.936546	898.058869	13.057280
20.774399	897.099075	13.062285
21.082433	911.487931	13.067290
20.874438	893.653029	13.072295
20.766447	898.215342	13.077299
20.890483	896.591696	13.082304
20.746329	886.871628	13.087309
20.562090	905.817839	13.092314
20.994219	893.768004	13.097319
20.885999	914.711274	13.102323
20.740229	893.873186	13.107328
20.640636	889.411808	13.112333
20.495117	900.261531	13.117338
21.100683	901.724662	13.122343
20.772505	911.802381	13.127347
20.849251	902.887643	13.132352
20.896215	908.261086	13.137357
20.598549	900.478468	13.142362
20.635849	904.459331	13.147367
20.468783	906.018885	13.152371
20.641073	908.990979	13.157376
20.908843	902.977529	13.162381
20.681895	903.991509	13.167386
20.811244	905.418625	13.172391
20.908488	899.984344	13.177395
20.890655	907.325253	13.182400
20.768200	895.564157	13.187405
20.644061	911.024952	13.192410
20.898054	903.684236	13.197415
20.641140	910.629588	13.202419
20.714415	899.573758	13.207424
20.789861	914.832401	13.212429
20.930768	898.747578	13.217434
21.031152	897.189209	13.222439
20.633501	902.750268	13.227443
21.088382	900.632275	13.232448
21.131612	909.196705	13.237453
20.852014	890.072154	13.242458
20.844125	881.112577	13.247463
20.720524	874.789375	13.252467
20.977359	865.609377	13.257472
20.567485	876.122753	13.262477
20.769296	868.902349	13.267482
20.775337	864.739542	13.272487
20.633056	878.085210	13.277491
20.601671	870.189170	13.282496
20.730030	880.515770	13.287501
21.147608	890.513954	13.292506
21.032535	892.237114	13.297511
20.382219	883.450969	13.302515
20.702043	867.640439	13.307520
20.564503	888.604118	13.312525
20.659857	904.534556	13.317530
20.918099	889.522354	13.322535
20.986814	908.811448	13.327539
21.059016	909.249400	13.332544
20.924921	897.856038	13.337549
20.654093	879.012395	13.342554
20.637069	877.726661	13.347559
20.758066	893.041098	13.352563
20.777406	887.231292	13.357568
20.945289	891.946734	13.362573
20.880281	893.056319	13.367578
20.837416	890.218148	13.372583
20.757873	882.514298	13.377587
20.630962	891.074313	13.382592
20.919411	880.865753	13.387597
20.662190	887.043116	13.392602
20.744708	882.951690	13.397607
20.411175	888.808465	13.402611
20.776702	896.261699	13.407616
21.046150	912.375704	13.412621
20.796265	901.270484	13.417626
21.002658	890.808482	13.422631
20.642825	884.707469	13.427635
20.889444	895.939374	13.432640
20.690613	891.356620	13.437645
20.762366	894.940875	13.442650
20.740510	886.174347	13.447655
20.598944	893.503442	13.452659
20.820478	903.271112	13.457664
21.145189	908.428355	13.462669
20.835452	906.599485	13.467674
20.827167	893.306205	13.472679
20.853445	886.850275	13.477683
20.939017	889.232183	13.482688
20.856037	890.436103	13.487693
20.767033	887.199988	13.492698
20.829135	883.204865	13.497703
20.447050	892.318124	13.502707
20.671389	887.967518	13.507712
20.560865	886.501141	13.512717
20.827404	890.986367	13.517722
21.032246	880.407918	13.522727
20.894705	885.337663	13.527731
20.744581	882.196459	13.532736
20.623600	886.705644	13.537741
20.466808	893.668136	13.542746
20.951533	899.370750	13.547751
20.878278	901.874193	13.552755
20.919817	887.098421	13.557760
20.775434	891.294351	13.562765
20.660630	900.011723	13.567770
20.711855	896.461484	13.572775
20.549724	896.712869	13.577779
20.925091	902.824037	13.582784
20.852325	904.587762	13.587789
21.178950	896.976828	13.592794
21.058109	888.937339	13.597799
20.723935	894.532428	13.602803
20.783594	886.837914	13.607808
21.139545	887.831467	13.612813
20.964063	897.209841	13.617818
20.797071	894.956054	13.622823
21.002069	894.010247	13.627827
20.534128	892.592991	13.632832
20.650443	892.798387	13.637837
20.788721	895.498341	13.642842
20.920960	888.847302	13.647847
20.707406	893.002222	13.652851
20.767158	897.503086	13.657856
20.664818	887.334772	13.662861
20.641022	887.676064	13.667866
20.899664	897.959818	13.672871
20.716413	903.073491	13.677875
20.622783	900.678684	13.682880
20.893891	895.773376	13.687885
20.903413	899.905334	13.692890
21.261604	891.338401	13.697895
20.948367	902.213299	13.702899
20.900071	903.903731	13.707904
21.162372	901.243982	13.712909
20.996111	902.817601	13.717914
21.039863	892.088206	13.722919
20.561702	898.755005	13.727923
21.118195	891.929057	13.732928
20.842474	880.498369	13.737933
20.385445	871.183053	13.742938
20.923422	892.409602	13.747943
20.849064	897.818163	13.752947
20.984971	893.010119	13.757952
20.631497	878.508685	13.762957
20.503271	884.126118	13.767962
20.927947	892.003606	13.772967
20.881732	895.474204	13.777971
20.898908	886.775572	13.782976
20.868400	871.382061	13.787981
20.470677	874.586998	13.792986
21.025204	879.373240	13.797991
20.694811	881.704791	13.802995
20.826212	888.657587	13.808000
20.916828	878.463234	13.813005
20.258672	877.855385	13.818010
20.735919	887.486058	13.823015
20.710272	900.499310	13.828019
20.901832	902.643527	13.833024
21.029186	895.993265	13.838029
21.104700	900.046884	13.843034
20.942877	876.393177	13.848039
20.956397	870.767244	13.853043
20.797155	875.273065	13.858048
20.570948	876.398897	13.863053
20.833974	870.171736	13.868058
20.821633	875.359071	13.873063
20.954984	880.589407	13.878067
20.973058	868.063126	13.883072
20.531603	869.686942	13.888077
20.638661	875.284193	13.893082
20.709840	863.703564	13.898087
21.008942	873.124507	13.903091
20.624565	868.442035	13.908096
20.674701	861.608549	13.913101
20.423824	872.976560	13.918106
20.917229	880.328959	13.923111
20.903407	879.124721	13.928115
20.619775	871.046548	13.933120
21.049967	869.333070	13.938125
20.707887	873.338163	13.943130
20.851806	866.256312	13.948135
20.660844	865.785272	13.953139
20.812070	878.470653	13.958144
20.934050	863.926518	13.963149
20.700343	870.248366	13.968154
20.870289	870.604490	13.973159
21.051137	874.177647	13.978163
20.963291	871.652604	13.983168
20.937414	865.279124	13.988173
20.574144	874.253744	13.993178
20.852802	871.477844	13.998183
20.754325	866.558949	14.003187
20.854359	871.698395	14.008192
20.565026	883.296696	14.013210
20.644705	880.738824	14.018227
21.072842	873.097960	14.023245
20.704468	880.114248	14.028263
20.898480	872.877243	14.033280
20.606808	878.099050	14.038298
20.898253	885.637741	14.043315
20.844912	876.700411	14.048333
20.878048	881.914457	14.053351
20.949741	875.461456	14.058368
20.855432	869.543023	14.063386
20.463911	877.182776	14.068403
20.967647	895.253683	14.073421
21.135775	905.088235	14.078439
20.912597	902.495294	14.083456
21.134255	905.044445	14.088474
20.892560	913.281669	14.093491
20.947729	903.568811	14.098509
21.180171	910.693779	14.103527
21.160018	904.374965	14.108544
20.857365	915.160794	14.113562
21.110935	905.037188	14.118579
21.220426	905.291866	14.123597
21.194312	912.925266	14.128615
20.985515	914.379028	14.133632
21.108804	903.569909	14.138650
20.952225	909.567709	14.143667
21.061199	909.374154	14.148685
21.034192	909.749704	14.153703
20.897353	912.905026	14.158720
21.475672	915.170775	14.163738
21.376480	931.412493	14.168755
21.619880	918.245097	14.173773
20.883460	924.338532	14.178791
21.034584	941.482588	14.183808
21.454558	940.061221	14.188826
21.051277	947.061086	14.193843
21.374883	946.474644	14.198861
21.203004	944.894416	14.203879
21.450640	949.913825	14.208896
21.399202	944.244930	14.213914
21.386904	940.789354	14.218931
21.650609	941.148425	14.223949
21.567530	945.279902	14.228967
21.191405	934.509517	14.233984
21.437762	943.928920	14.239002
21.453176	937.854532	14.244019
21.500255	945.320544	14.249037
21.807343	952.537448	14.254055
22.180450	960.612145	14.259072
22.042387	948.395906	14.264090
21.895371	955.896027	14.269107
21.863228	949.289666	14.274125
21.672845	947.448118	14.279143
21.660058	950.885686	14.284160
21.884287	953.231513	14.289178
21.590001	962.409967	14.294195
21.622855	949.597024	14.299213
21.574036	948.571329	14.304231
21.467948	950.656805	14.309248
22.066573	949.225820	14.314266
21.727693	953.380795	14.319283
21.888746	956.713558	14.324301
21.735819	951.024668	14.329319
21.790942	970.908578	14.334336
22.191858	978.679971	14.339354
21.866749	989.036849	14.344371
22.126997	984.792169	14.349389
22.036594	991.408666	14.354407
21.748925	981.948641	14.359424
21.955953	983.290468	14.364442
21.878775	979.709949	14.369459
22.237001	977.115499	14.374477
22.063378	978.176687	14.379495
21.941298	986.034647	14.384512
22.244736	979.097892	14.389530
21.851777	987.680185	14.394547
22.247618	978.535867	14.399565
22.091798	978.460051	14.404583
22.150610	990.294133	14.409600
22.473153	976.557203	14.414618
22.551220	981.362993	14.419635
22.287266	980.261495	14.424653
22.362987	982.470563	14.429671
22.152913	989.546599	14.434688
22.342925	979.761846	14.439706
22.395846	989.449661	14.444723
22.341964	977.639974	14.449741
22.434019	984.628493	14.454759
22.177840	987.741516	14.459776
22.325687	986.476808	14.464794
22.129104	986.646596	14.469811
22.430989	988.213970	14.474829
22.401673	989.628101	14.479847
22.176350	980.438135	14.484864
22.377202	983.756691	14.489882
22.344653	994.988715	14.494899
22.834804	1007.817394	14.499917
23.100514	1011.293928	14.504935
22.893052	1002.108965	14.509952
22.974479	980.908629	14.514970
22.493979	990.480174	14.519987
22.749124	971.822500	14.525005
23.051383	978.978839	14.530023
22.541660	982.382414	14.535040
22.763511	969.879088	14.540058
22.489762	981.157437	14.545075
22.474566	977.170626	14.550093
22.744963	974.774230	14.555111
22.299334	988.107653	14.560128
22.922789	997.043796	14.565146
22.812539	1002.971323	14.570163
22.799555	1010.398184	14.575181
23.433901	1011.448485	14.580199
23.059514	1007.880756	14.585216
23.206355	977.384295	14.590234
23.106378	975.128771	14.595251
22.922772	977.780326	14.600269
23.225252	974.759034	14.605287
22.737527	980.510801	14.610304
23.257453	970.374556	14.615322
23.248337	981.782159	14.620339
23.117073	980.178146	14.625357
23.286938	976.312830	14.630375
22.908004	974.713714	14.635392
23.324543	972.353785	14.640410
23.052707	975.810653	14.645427
23.016789	989.685925	14.650445
22.885324	974.854210	14.655463
22.872231	979.984428	14.660480
23.119875	975.153443	14.665498
22.940753	989.466839	14.670515
22.971004	1001.514700	14.675533
22.964156	1004.564364	14.680551
22.936464	1012.128854	14.685568
23.423454	1010.064427	14.690586
23.425647	1016.640998	14.695603
23.173140	1009.265928	14.700621
23.479583	1018.696247	14.705639
23.085387	1009.460837	14.710656
23.427828	1014.792342	14.715674
23.276806	1008.675255	14.720691
23.269300	1011.492214	14.725709
23.460447	1009.832055	14.730727
23.441957	1014.527413	14.735744
23.749238	1011.615461	14.740762
23.355171	1012.025963	14.745779
23.565282	1014.852258	14.750797
23.510440	1020.490953	14.755815
23.360889	1023.217310	14.760832
23.946981	1027.254664	14.765850
23.551177	1020.454585	14.770867
23.159892	1014.191771	14.775885
23.612900	1021.784990	14.780903
23.755355	1036.073883	14.785920
23.892610	1042.248246	14.790938
24.341850	1032.178288	14.795955
24.084333	1033.622528	14.800973
24.013791	1013.833813	14.805991
23.755192	1019.379162	14.811008
23.780466	1006.977943	14.816026
23.790397	1001.830928	14.821043
23.572008	1004.277247	14.826061
24.153071	990.099518	14.831079
23.736940	1001.792280	14.836096
23.644114	1005.926902	14.841114
23.841091	1016.349968	14.846131
24.196116	1029.684718	14.851149
24.320563	1022.046596	14.856167
23.984714	1015.449318	14.861184
24.195960	1001.793037	14.866202
23.915601	1000.934830	14.871219
23.945062	1005.567481	14.876237
24.306135	1006.049452	14.881255
24.155353	1005.717998	14.886272
24.010626	1003.595451	14.891290
24.108152	1009.678607	14.896307
24.184429	1015.968078	14.901325
24.331419	1022.156610	14.906343
24.075573	1027.220169	14.911360
24.452599	1021.986281	14.916378
23.992189	1018.334741	14.921395
24.311096	1026.108229	14.926413
24.563313	1022.965954	14.931431
24.508938	1021.744508	14.936448
24.334160	1020.860022	14.941466
24.419498	1009.729683	14.946483
24.228191	1015.434187	14.951501
24.480276	1014.953533	14.956519
24.410639	1017.170059	14.961536
24.441778	1024.182471	14.966554
24.578966	1025.538587	14.971571
24.506200	1032.496787	14.976589
24.898438	1021.440188	14.981607
24.531875	1012.162616	14.986624
24.549614	993.954918	14.991642
24.577887	1002.847566	14.996659
24.243196	1008.029089	15.001677
24.669094	1023.484008	15.006695
24.783587	1032.158426	15.011712
24.903559	1025.150237	15.016730
25.007966	1023.269527	15.021747
24.382982	1011.824610	15.026765
24.802009	1003.241303	15.031783
25.048202	1031.373771	15.036800
24.893319	1010.187487	15.041818
24.832462	999.102497	15.046835
24.493603	1011.827446	15.051853
24.721550	1014.699662	15.056871
24.783239	1027.098039	15.061888
24.615031	1028.562641	15.066906
24.640139	1028.717521	15.071923
24.539314	1032.666233	15.076941
24.680702	1028.888818	15.081959
24.719527	1037.789243	15.086976
24.528525	1031.958526	15.091994
24.951488	1022.333221	15.097011
24.825192	1032.884939	15.102029
25.072139	1045.110637	15.107047
25.185840	1063.597899	15.112064
25.212848	1067.026001	15.117082
25.353453	1055.823891	15.122099
25.159295	1052.312349	15.127117
25.264329	1037.178577	15.132135
25.115711	1032.336841	15.137152
24.952917	1036.669824	15.142170
25.111608	1050.970300	15.147187
25.276496	1062.032457	15.152205
25.653176	1054.866903	15.157223
25.229346	1051.149744	15.162240
25.238937	1048.978981	15.167258
25.249886	1052.131210	15.172275
25.261112	1063.477431	15.177293
25.417849	1063.512214	15.182311
25.600000	1068.104800	15.187328
25.361402	1067.947802	15.192346
25.480208	1066.396704	15.197363
25.299473	1072.075948	15.202381
25.504589	1061.558834	15.207399
25.536173	1069.126483	15.212416
25.591695	1073.644885	15.217434
25.859616	1061.477057	15.222451
25.561664	1056.511265	15.227469
26.136105	1060.990943	15.232487
25.983983	1056.535156	15.237504
25.486952	1038.231751	15.242522
25.349045	1029.463546	15.247539
25.231164	1048.181211	15.252557
25.664770	1058.115100	15.257575
25.367827	1067.614946	15.262592
25.626102	1061.449860	15.267610
25.618380	1063.362358	15.272627
25.536661	1069.121764	15.277645
25.830152	1056.352102	15.282663
26.118446	1062.530698	15.287680
25.907289	1066.317689	15.292698
26.068129	1060.138255	15.297715
25.776881	1068.391336	15.302733
26.066413	1059.160102	15.307751
25.943701	1065.509647	15.312768
25.727568	1063.302524	15.317786
26.123975	1057.008440	15.322803
25.812391	1056.702633	15.327821
25.784051	1052.944417	15.332839
25.917991	1060.453264	15.337856
26.107496	1083.433687	15.342874
26.612023	1079.423731	15.347891
26.038328	1075.153156	15.352909
26.305862	1064.802267	15.357927
26.194834	1054.680080	15.362944
25.783795	1056.188134	15.367962
26.290174	1071.517009	15.372979
26.410466	1086.171289	15.377997
26.395211	1084.734382	15.383015
26.712903	1083.283697	15.388032
26.535193	1060.999841	15.393050
26.642226	1053.911902	15.398067
26.190940	1061.031163	15.403085
26.513920	1047.877700	15.408103
26.589598	1052.616253	15.413120
26.511050	1059.720109	15.418138
26.848052	1051.159296	15.423155
26.841035	1045.852943	15.428173
26.366936	1053.087526	15.433191
26.704326	1051.319092	15.438208
26.317207	1054.725152	15.443226
26.694427	1056.588837	15.448243
26.444001	1057.124296	15.453261
26.543324	1049.413087	15.458279
26.573330	1047.069179	15.463296
26.601170	1049.237129	15.468314
26.731425	1051.258182	15.473331
26.501592	1058.733812	15.478349
26.726996	1059.311358	15.483367
26.649613	1053.578917	15.488384
26.790406	1054.396477	15.493402
26.828084	1066.265453	15.498419
26.938479	1073.770198	15.503437
27.088957	1069.758510	15.508455
26.963957	1062.348919	15.513472
26.835979	1058.221195	15.518490
26.911870	1044.182189	15.523507
26.569300	1063.752124	15.528525
26.978361	1072.739814	15.533543
27.146397	1076.574869	15.538560
26.840277	1086.441139	15.543578
27.040131	1076.517896	15.548595
27.216160	1090.389347	15.553613
27.063708	1076.589654	15.558631
27.119447	1084.471216	15.563648
26.934738	1088.785687	15.568666
27.257593	1080.744648	15.573683
27.093694	1089.208668	15.578701
27.053191	1089.114458	15.583719
27.232022	1085.206785	15.588736
26.948383	1084.388422	15.593754
27.179620	1072.438799	15.598771
27.279905	1086.649523	15.603789
27.428086	1079.965577	15.608807
27.293901	1082.780731	15.613824
27.174879	1081.078798	15.618842
27.352862	1074.764487	15.623859
27.420394	1079.542102	15.628877
27.359595	1099.126920	15.633895
27.617257	1098.816838	15.638912
27.578349	1106.148780	15.643930
27.828824	1105.654222	15.648947
27.859364	1092.659048	15.653965
27.896780	1076.626792	15.658983
27.754805	1076.479552	15.664000
27.429123	1077.841858	15.669018
27.594983	1071.441391	15.674035
27.607010	1076.651010	15.679053
27.438127	1075.441530	15.684071
27.801959	1079.139963	15.689088
27.745118	1101.338571	15.694106
28.004840	1102.830884	15.699123
28.125482	1087.428723	15.704141
27.692718	1081.241709	15.709159
27.777355	1076.098482	15.714176
27.378488	1081.302850	15.719194
27.790023	1095.158767	15.724211
27.982914	1105.629741	15.729229
27.752094	1104.755761	15.734247
28.035895	1102.983284	15.739264
27.896789	1108.331852	15.744282
27.929720	1108.938525	15.749299
27.758453	1108.880902	15.754317
27.890639	1104.285372	15.759335
27.917521	1100.523055	15.764352
27.999818	1108.768490	15.769370
28.357324	1099.907070	15.774387
28.135531	1107.499421	15.779405
28.231924	1106.691231	15.784423
28.326080	1096.968880	15.789440
28.320852	1103.716564	15.794458
28.407320	1101.951966	15.799475
28.404479	1106.312942	15.804493
28.218716	1103.608601	15.809511
28.414323	1106.275203	15.814528
28.092625	1106.520004	15.819546
28.406945	1099.111113	15.824563
28.656869	1087.150632	15.829581
28.439032	1104.743846	15.834599
28.378815	1097.607055	15.839616
28.362499	1107.620604	15.844634
28.714830	1106.600130	15.849651
28.759768	1105.010472	15.854669
28.399956	1113.787330	15.859687
28.647204	1112.033267	15.864704
28.698697	1125.119209	15.869722
28.698442	1125.561286	15.874739
28.996802	1127.571268	15.879757
28.747257	1110.771471	15.884775
28.790342	1097.223721	15.889792
28.412589	1099.962893	15.894810
28.712689	1107.948642	15.899827
29.167943	1114.629180	15.904845
28.953784	1126.648486	15.909863
29.281993	1109.272039	15.914880
28.713771	1111.456414	15.919898
28.797400	1095.537892	15.924915
28.907285	1107.508646	15.929933
28.863527	1118.497156	15.934951
28.797989	1116.961298	15.939968
29.238764	1122.201652	15.944986
29.319913	1121.114315	15.950003
29.483533	1125.494367	15.955021
28.950087	1111.896981	15.960039
29.200588	1095.372958	15.965056
29.043273	1103.702226	15.970074
29.051650	1105.830817	15.975091
29.238342	1113.394201	15.980109
29.320719	1121.520078	15.985127
29.245472	1122.389403	15.990144
29.286929	1123.612930	15.995162
29.468544	1114.262018	16.000179
29.611915	1124.712589	16.005197
29.272642	1108.518575	16.010215
29.264154	1098.057526	16.015232
29.485174	1113.897585	16.020250
29.515488	1122.162331	16.025267
29.728968	1117.437424	16.030285
29.333480	1112.592562	16.035303
29.311439	1109.132208	16.040320
29.340026	1127.395596	16.045338
29.645948	1115.489083	16.050355
29.553436	1119.140758	16.055373
29.183295	1131.260453	16.060391
29.645736	1117.210062	16.065408
29.679285	1125.494743	16.070426
29.521804	1122.999824	16.075443
29.577168	1122.838413	16.080461
29.375999	1123.787598	16.085479
29.358593	1124.378705	16.090496
29.654675	1132.303759	16.095514
29.816088	1151.101282	16.100531
29.946453	1161.572831	16.105549
29.581622	1161.953503	16.110567
30.032841	1161.217710	16.115584
29.883400	1166.226592	16.120602
29.825691	1157.750693	16.125619
29.922504	1155.076780	16.130637
29.825634	1156.718784	16.135655
29.890133	1148.868355	16.140672
29.747531	1163.202839	16.145690
29.943526	1157.903393	16.150707
30.110479	1154.771543	16.155725
29.959983	1162.610534	16.160743
30.154757	1146.856704	16.165760
30.047877	1148.899862	16.170778
30.147185	1164.594217	16.175795
30.673094	1167.582539	16.180813
30.592321	1162.059813	16.185831
30.340829	1150.665330	16.190848
30.412009	1147.457519	16.195866
30.528493	1149.432018	16.200883
30.604900	1141.996555	16.205901
30.272698	1156.918136	16.210919
30.583038	1143.242773	16.215936
30.585113	1143.846504	16.220954
30.367534	1142.589728	16.225971
30.384857	1137.315640	16.230989
30.405672	1142.745682	16.236007
30.616229	1146.142955	16.241024
30.621928	1149.868638	16.246042
30.446493	1159.811644	16.251059
31.071682	1168.640652	16.256077
30.544824	1161.048132	16.261095
31.085318	1155.475086	16.266112
31.031594	1148.341953	16.271130
30.578765	1147.934398	16.276147
31.139147	1135.606603	16.281165
30.785515	1135.008617	16.286183
30.847349	1143.501161	16.291200
30.860011	1140.368754	16.296218
30.963302	1145.107653	16.301235
30.996573	1142.739612	16.306253
30.700469	1150.951040	16.311271
31.077868	1148.871041	16.316288
30.898546	1157.320256	16.321306
31.051974	1174.682876	16.326323
31.371929	1175.972103	16.331341
31.361365	1171.117741	16.336359
31.184888	1148.187023	16.341376
31.253016	1148.372796	16.346394
30.969874	1145.558133	16.351411
31.422122	1158.034334	16.356429
31.112079	1162.755790	16.361447
31.110985	1174.313280	16.366464
31.289904	1167.819451	16.371482
31.271801	1174.388319	16.376499
31.375592	1168.526260	16.381517
31.224293	1181.270207	16.386535
31.377378	1181.928507	16.391552
31.254754	1180.755687	16.396570
30.927888	1176.516501	16.401587
31.326980	1171.099712	16.406605
30.767066	1171.755324	16.411623
31.667737	1188.913836	16.416640
32.032576	1204.638245	16.421658
31.830978	1191.467643	16.426675
31.948928	1176.457510	16.431693
31.971570	1169.277580	16.436711
31.941612	1169.198991	16.441728
32.048521	1162.306080	16.446746
31.665776	1165.211232	16.451763
31.993663	1163.098227	16.456781
31.776896	1175.371253	16.461799
31.933555	1166.924081	16.466816
31.911127	1165.280665	16.471834
31.970362	1166.638217	16.476851
32.171610	1168.147729	16.481869
31.947599	1166.788154	16.486887
32.170184	1158.118109	16.491904
32.171311	1163.848608	16.496922
32.007804	1165.559445	16.501939
32.387912	1158.149470	16.506957
31.919776	1161.239704	16.511975
32.135400	1166.807002	16.516992
32.154827	1165.729506	16.522010
32.212947	1163.854588	16.527027
32.006378	1160.675343	16.532045
32.113088	1171.309551	16.537063
32.015157	1158.561329	16.542080
32.089897	1161.034856	16.547098
31.827209	1169.060062	16.552115
32.417837	1183.507289	16.557133
32.185760	1196.828863	16.562151
32.584346	1197.105080	16.567168
32.648706	1190.698728	16.572186
32.521947	1206.863351	16.577203
32.833964	1198.037442	16.582221
32.763502	1199.038146	16.587239
32.540398	1190.149722	16.592256
32.510267	1194.025853	16.597274
32.083625	1201.918346	16.602291
32.086338	1188.021438	16.607309
32.148214	1193.990804	16.612327
32.155190	1197.011561	16.617344
32.692327	1201.457908	16.622362
32.656724	1214.853559	16.627379
32.950535	1221.309777	16.632397
32.810282	1225.927093	16.637415
33.049701	1212.670401	16.642432
33.327746	1220.867376	16.647450
32.943056	1209.489372	16.652467
33.003604	1206.396505	16.657485
33.051404	1201.702714	16.662503
32.934222	1213.200097	16.667520
33.391322	1209.721503	16.672538
33.173913	1213.120980	16.677555
33.148070	1203.117240	16.682573
33.025225	1203.506510	16.687591
33.411639	1207.464077	16.692608
33.107037	1200.243514	16.697626
33.256761	1207.227662	16.702643
33.149417	1203.818644	16.707661
33.473629	1209.739884	16.712679
33.238121	1213.493043	16.717696
33.209833	1214.575113	16.722714
33.359068	1214.917843	16.727731
33.367716	1211.713699	16.732749
33.553359	1209.802705	16.737767
33.644886	1216.372984	16.742784
33.466201	1214.007276	16.747802
33.435608	1211.199512	16.752819
33.849644	1210.221102	16.757837
33.772313	1213.014629	16.762855
33.583847	1220.546666	16.767872
33.860518	1213.601486	16.772890
33.673799	1214.795344	16.777907
33.810499	1204.600506	16.782925
33.822322	1211.351813	16.787943
33.689450	1215.859407	16.792960
33.803673	1207.728874	16.797978
33.614046	1212.099223	16.802995
33.389524	1211.508957	16.808013
33.900505	1203.914486	16.813031
33.991641	1203.695458	16.818048
33.711868	1206.840605	16.823066
33.600637	1211.780485	16.828083
33.727709	1202.637996	16.833101
33.838239	1208.717589	16.838119
34.000088	1223.170319	16.843136
34.068067	1228.507926	16.848154
33.763892	1242.784884	16.853171
34.119579	1234.241434	16.858189
34.346601	1232.388334	16.863207
34.405729	1242.522081	16.868224
34.541806	1238.194097	16.873242
34.738508	1233.063616	16.878259
34.833363	1222.288685	16.883277
34.700809	1205.396183	16.888295
34.361898	1200.937108	16.893312
34.749385	1200.813963	16.898330
34.504726	1211.044905	16.903347
34.419143	1199.271555	16.908365
34.406710	1204.631416	16.913383
34.187757	1205.445012	16.918400
34.581710	1202.907748	16.923418
34.698747	1220.044986	16.928435
34.912229	1219.021482	16.933453
34.915336	1208.218721	16.938471
34.500000	1208.813521	16.943488
34.669584	1204.166375	16.948506
34.701358	1231.137898	16.953523
34.816718	1224.976661	16.958541
34.897944	1231.160041	16.963559
34.558996	1236.601092	16.968576
34.869324	1229.110185	16.973594
34.678513	1236.502601	16.978611
34.952282	1225.343618	16.983629
35.210545	1231.528650	16.988647
34.983416	1239.806994	16.993664
35.016804	1231.111237	16.998682
35.206530	1239.010840	17.003699
35.216900	1224.585696	17.008717
35.186335	1235.270161	17.013735
34.825346	1233.499831	17.018752
35.017378	1232.984704	17.023770
34.820184	1243.893958	17.028787
34.897144	1233.163559	17.033805
35.065963	1245.671670	17.038823
35.189430	1257.988817	17.043840
35.642884	1263.739239	17.048858
35.230450	1272.238284	17.053875
35.454231	1269.146112	17.058893
35.482829	1261.556186	17.063911
35.320121	1264.509636	17.068928
35.545135	1266.932471	17.073946
35.566655	1270.065758	17.078963
35.757530	1265.152494	17.083981
35.718567	1259.030800	17.088999
35.438720	1272.124887	17.094016
35.632519	1252.938646	17.099034
35.856197	1261.076674	17.104051
36.001138	1264.239040	17.109069
36.216031	1256.158494	17.114087
35.633694	1263.688089	17.119104
35.916265	1261.345551	17.124122
35.720553	1257.703642	17.129139
35.778445	1252.485178	17.134157
35.662535	1254.669008	17.139175
35.632148	1256.469525	17.144192
36.067694	1256.132642	17.149210
36.029196	1248.074423	17.154227
35.780534	1256.985441	17.159245
36.122671	1262.827550	17.164263
36.148859	1281.035670	17.169280
36.342606	1282.846849	17.174298
36.089033	1274.587743	17.179315
36.067888	1277.151304	17.184333
36.276838	1276.845055	17.189351
36.267462	1287.416063	17.194368
36.467155	1287.602092	17.199386
36.549641	1285.725631	17.204403
36.155238	1289.049531	17.209421
36.456454	1279.375047	17.214439
36.215323	1285.487164	17.219456
36.250047	1287.072013	17.224474
36.150219	1288.266176	17.229491
36.351818	1291.716037	17.234509
36.517901	1293.606351	17.239527
36.296553	1304.197021	17.244544
36.775968	1305.070705	17.249562
37.067333	1311.554883	17.254579
37.095557	1319.297025	17.259597
37.059048	1305.763348	17.264615
36.831029	1287.085588	17.269632
37.076890	1278.842782	17.274650
36.984342	1275.160032	17.279667
36.896476	1277.916711	17.284685
37.132448	1272.352863	17.289703
37.117843	1282.234121	17.294720
36.961514	1282.903235	17.299738
37.066283	1280.488375	17.304755
37.085196	1277.727761	17.309773
37.672365	1281.456696	17.314791
37.248260	1284.251272	17.319808
37.074251	1273.562444	17.324826
37.316901	1265.264314	17.329843
37.227451	1267.960680	17.334861
37.378586	1272.814691	17.339879
37.098542	1278.819749	17.344896
37.125568	1278.533077	17.349914
37.377660	1289.152837	17.354931
37.554729	1297.778894	17.359949
37.599903	1292.144006	17.364967
37.416375	1302.030196	17.369984
37.138076	1298.008964	17.375002
37.689644	1297.846279	17.380019
37.631141	1300.410296	17.385037
37.835817	1297.970060	17.390055
37.598725	1304.111429	17.395072
37.874322	1302.495973	17.400090
37.895283	1300.325719	17.405107
37.640728	1294.780320	17.410125
38.054712	1292.669297	17.415143
37.855034	1297.492748	17.420160
37.705750	1288.716762	17.425178
38.068082	1298.420718	17.430195
37.935591	1304.806535	17.435213
38.308708	1296.941412	17.440231
38.224795	1299.860279	17.445248
37.835042	1308.435955	17.450266
38.244242	1296.346863	17.455283
37.620603	1302.458642	17.460301
38.037854	1305.240948	17.465319
37.839099	1303.744407	17.470336
37.903748	1295.672070	17.475354
38.098970	1302.634850	17.480371
37.781458	1310.038073	17.485389
38.196616	1314.762682	17.490407
38.390475	1331.174407	17.495424
38.563412	1332.527211	17.500442
38.818878	1325.734016	17.505459
38.473272	1330.170964	17.510477
38.564529	1329.773370	17.515495
38.363246	1322.261763	17.520512
38.323718	1315.763382	17.525530
38.537106	1317.351987	17.530547
38.289349	1322.423009	17.535565
38.689989	1322.076749	17.540583
38.609008	1324.244793	17.545600
38.605483	1325.949795	17.550618
38.800308	1326.133454	17.555635
38.660504	1322.679246	17.560653
38.798242	1313.380824	17.565671
38.820328	1324.270896	17.570688
38.782848	1340.508735	17.575706
39.118459	1342.714949	17.580723
39.007487	1349.717935	17.585741
39.442411	1342.957461	17.590759
39.454671	1346.586189	17.595776
38.974488	1342.052070	17.600794
39.053102	1321.435300	17.605811
39.470257	1340.367680	17.610829
39.438304	1328.543197	17.615847
39.417021	1321.471661	17.620864
39.237755	1312.591113	17.625882
39.360360	1306.534082	17.630899
39.061718	1316.102789	17.635917
39.222707	1320.795576	17.640935
39.261926	1336.488690	17.645952
38.967985	1336.474226	17.650970
39.618142	1339.526144	17.655987
38.924800	1339.263123	17.661005
39.324684	1344.988301	17.666023
39.238397	1342.888630	17.671040
39.534601	1346.972313	17.676058
40.035177	1357.638226	17.681075
39.787069	1366.929122	17.686093
40.111485	1354.107862	17.691111
40.276594	1335.332731	17.696128
40.037603	1325.887525	17.701146
39.972622	1327.190182	17.706163
40.069653	1330.350766	17.711181
40.333169	1329.821088	17.716199
40.410162	1328.888561	17.721216
40.317374	1329.256523	17.726234
40.255995	1323.870646	17.731251
40.058639	1322.711305	17.736269
40.467490	1318.544293	17.741287
40.387820	1319.954689	17.746304
40.415329	1325.089566	17.751322
40.178386	1318.692671	17.756339
40.233184	1336.623368	17.761357
40.359152	1327.932451	17.766375
40.189898	1323.568979	17.771392
40.097875	1327.700417	17.776410
40.386556	1319.803916	17.781427
40.358785	1325.023904	17.786445
40.572891	1324.297606	17.791463
40.636136	1319.586371	17.796480
40.297262	1318.738261	17.801498
40.626353	1324.677649	17.806515
40.576710	1328.582097	17.811533
40.378001	1320.856141	17.816551
40.476415	1328.075055	17.821568
40.691543	1347.950481	17.826586
41.285420	1342.769202	17.831603
40.909906	1361.750165	17.836621
40.883624	1351.177722	17.841639
40.755295	1353.713558	17.846656
41.030707	1356.081179	17.851674
41.314065	1355.023712	17.856691
40.873682	1357.853146	17.861709
41.043080	1348.577967	17.866727
41.219629	1353.077941	17.871744
41.072949	1358.806921	17.876762
41.256982	1343.355052	17.881779
41.076588	1349.715493	17.886797
41.304331	1335.713337	17.891815
41.229771	1346.607042	17.896832
41.235518	1353.951650	17.901850
41.283978	1354.415067	17.906867
41.507929	1346.157627	17.911885
41.295367	1345.884783	17.916903
41.326518	1347.964158	17.921920
41.244049	1352.382740	17.926938
41.571748	1348.128772	17.931955
41.435421	1352.938205	17.936973
41.608794	1356.099203	17.941991
41.640936	1360.367370	17.947008
41.599245	1376.831659	17.952026
41.747877	1371.950266	17.957043
41.646754	1377.562659	17.962061
41.518529	1384.861794	17.967079
41.576170	1381.258100	17.972096
41.618517	1378.677780	17.977114
41.840114	1375.219405	17.982131
41.449541	1377.637401	17.987149
41.668225	1392.128429	17.992167
42.279253	1399.114606	17.997184
42.364527	1415.168562	18.002202
42.467719	1413.919593	18.007219
42.348051	1405.790859	18.012237
42.059374	1385.485057	18.017255
42.480852	1392.959231	18.022272
42.217830	1397.767648	18.027290
42.842572	1406.128881	18.032307
42.337140	1394.303564	18.037325
42.176984	1381.072694	18.042343
42.418705	1381.579223	18.047360
42.361021	1401.357441	18.052378
42.703512	1399.305786	18.057395
42.747307	1403.145799	18.062413
42.788675	1402.049843	18.067431
42.972317	1403.189366	18.072448
43.028119	1403.603634	18.077466
42.910124	1395.399916	18.082483
42.666098	1391.114419	18.087501
42.825143	1398.758657	18.092519
42.861914	1407.088605	18.097536
42.711269	1404.057695	18.102554
42.873807	1403.948404	18.107571
42.757827	1403.767912	18.112589
42.927329	1402.951979	18.117607
43.073694	1395.353426	18.122624
42.667082	1402.379992	18.127642
42.980879	1397.045941	18.132659
42.861997	1403.723012	18.137677
42.816542	1403.741279	18.142695
43.087657	1407.703921	18.147712
43.183856	1428.125410	18.152730
43.348818	1434.189338	18.157747
43.349792	1429.077421	18.162765
43.494698	1428.613064	18.167783
43.590289	1424.116082	18.172800
43.237093	1436.342656	18.177818
43.719621	1425.155732	18.182835
43.455082	1432.258757	18.187853
43.411924	1416.492245	18.192871
43.511665	1421.702156	18.197888
43.420304	1427.287841	18.202906
43.874354	1423.564283	18.207923
43.995441	1422.273918	18.212941
43.807324	1425.564161	18.217959
43.674663	1427.276400	18.222976
43.618389	1423.998403	18.227994
43.807753	1428.775580	18.233011
44.250344	1443.647032	18.238029
44.262542	1436.295595	18.243047
44.184176	1427.112581	18.248064
44.186153	1421.713417	18.253082
44.314262	1414.706889	18.258099
44.056873	1413.435987	18.263117
44.012300	1420.731237	18.268135
44.349530	1426.657571	18.273152
44.466942	1438.319072	18.278170
44.682290	1446.798321	18.283187
44.578957	1438.527744	18.288205
44.432615	1433.895518	18.293223
44.483600	1423.150244	18.298240
44.533485	1443.605098	18.303258
44.862622	1448.260098	18.308275
44.592816	1422.733278	18.313293
44.466830	1437.710350	18.318311
44.936033	1445.488412	18.323328
44.754038	1448.114624	18.328346
44.883618	1446.262881	18.333363
44.996484	1442.664522	18.338381
44.630606	1454.412553	18.343399
44.855717	1443.177003	18.348416
44.887113	1453.498587	18.353434
44.635979	1458.747167	18.358451
44.993218	1454.047991	18.363469
44.829709	1456.966998	18.368487
45.007198	1442.822524	18.373504
44.731741	1452.928766	18.378522
45.074023	1454.896397	18.383539
45.281366	1449.661893	18.388557
45.045922	1460.670222	18.393575
45.145553	1464.819112	18.398592
45.224670	1475.438281	18.403610
45.293681	1475.528746	18.408627
45.188162	1470.569085	18.413645
45.070241	1481.940162	18.418663
45.481635	1466.561232	18.423680
45.273066	1471.304356	18.428698
45.513079	1476.867099	18.433715
45.425320	1480.684854	18.438733
45.838355	1493.584473	18.443751
45.874597	1487.950933	18.448768
45.961488	1489.254553	18.453786
45.606721	1475.550455	18.458803
45.952145	1492.448661	18.463821
45.654743	1497.655082	18.468839
46.108193	1496.082030	18.473856
45.945852	1511.997038	18.478874
46.222825	1503.401489	18.483891
46.392844	1495.656746	18.488909
46.109960	1502.245181	18.493927
46.305090	1504.443151	18.498944
46.155517	1509.626786	18.503962
46.141786	1505.876347	18.508979
46.474227	1491.994203	18.513997
46.271586	1498.827041	18.519015
46.605205	1491.775902	18.524032
46.089705	1497.643200	18.529050
46.077081	1497.138681	18.534067
46.297480	1493.044937	18.539085
46.110547	1501.919515	18.544103
46.388472	1495.574140	18.549120
46.531596	1495.354682	18.554138
46.498780	1511.906589	18.559155
47.126477	1523.203616	18.564173
46.974500	1519.722986	18.569191
46.918356	1505.170524	18.574208
46.626752	1504.049796	18.579226
47.171811	1510.116846	18.584243
47.250544	1520.090351	18.589261
46.875921	1514.315465	18.594279
47.076988	1522.288138	18.599296
47.189955	1528.383209	18.604314
47.090179	1533.179005	18.609331
47.121636	1531.103788	18.614349
47.135234	1530.246644	18.619367
47.025228	1519.777885	18.624384
47.035578	1527.532427	18.629402
46.998901	1520.401111	18.634419
47.433648	1516.410035	18.639437
47.346117	1530.955545	18.644455
47.352367	1527.695083	18.649472
47.283065	1530.617171	18.654490
47.535804	1524.288385	18.659507
47.778761	1526.628175	18.664525
47.552416	1553.377182	18.669543
47.724346	1552.582091	18.674560
47.698843	1560.516197	18.679578
47.643761	1566.503584	18.684595
47.881129	1553.931999	18.689613
47.853667	1559.911046	18.694631
47.918511	1556.473696	18.699648
47.970368	1551.792518	18.704666
48.051870	1560.031258	18.709683
48.135494	1560.134337	18.714701
47.915013	1558.307734	18.719719
47.990493	1562.134084	18.724736
48.144686	1550.068151	18.729754
47.873821	1556.899311	18.734771
47.994584	1556.106089	18.739789
47.884776	1563.794079	18.744807
47.971729	1556.390545	18.749824
48.274874	1575.829080	18.754842
48.456398	1566.653296	18.759859
48.412241	1572.085995	18.764877
48.585744	1575.062181	18.769895
48.337988	1566.568373	18.774912
48.260280	1568.689524	18.779930
48.192608	1585.139315	18.784947
48.845220	1580.849192	18.789965
48.627843	1595.237714	18.794983
49.119369	1604.901609	18.800000
48.947129	1601.354188	18.805018
48.943804	1599.065060	18.810035
49.346972	1597.398552	18.815053
49.010573	1582.922958	18.820071
49.366848	1568.626359	18.825088
49.364761	1560.769810	18.830106
49.032865	1564.083015	18.835123
48.944397	1560.356280	18.840141
49.142422	1577.865649	18.845159
49.391514	1584.450294	18.850176
49.637147	1591.355621	18.855194
49.706205	1588.917303	18.860211
49.865366	1573.018462	18.865229
49.497560	1563.056427	18.870247
49.776304	1560.403765	18.875264
49.692276	1561.024392	18.880282
49.488463	1551.166779	18.885299
49.825063	1546.993923	18.890317
49.842385	1547.878398	18.895335
49.625077	1553.545569	18.900352
49.842604	1561.196298	18.905370
49.891093	1575.155413	18.910387
50.025665	1574.361560	18.915405
49.794824	1586.995845	18.920423
49.625409	1576.705629	18.925440
50.188723	1573.591492	18.930458
49.825458	1581.360816	18.935475
49.952845	1585.299237	18.940493
49.751673	1587.438508	18.945511
49.976938	1579.673111	18.950528
49.875464	1580.885651	18.955546
50.174038	1596.179799	18.960563
50.718827	1603.909712	18.965581
50.721477	1606.103787	18.970599
50.930551	1588.416991	18.975616
50.819637	1576.857384	18.980634
50.491064	1572.670263	18.985651
50.744937	1569.553566	18.990669
50.782526	1569.264418	18.995687
51.003488	1566.791652	19.000704
51.140937	1564.101746	19.005722
50.877269	1571.095369	19.010739
51.123132	1560.427458	19.015757
50.903686	1568.099901	19.020775
51.156513	1565.338894	19.025792
51.424129	1557.400792	19.030810
51.171609	1570.883279	19.035827
51.245297	1558.970184	19.040845
51.255370	1560.993173	19.045863
51.430425	1553.009270	19.050880
51.615463	1558.205627	19.055898
51.055820	1560.783544	19.060915
51.341051	1555.689958	19.065933
51.635823	1557.061109	19.070951
51.666794	1555.723753	19.075968
51.426670	1567.652390	19.080986
51.423234	1564.299864	19.086003
51.311350	1555.441455	19.091021
51.512019	1554.180860	19.096039
51.266924	1561.335906	19.101056
51.420436	1556.459179	19.106074
51.372342	1562.933900	19.111091
51.705450	1555.444702	19.116109
51.685095	1567.881797	19.121127
51.336654	1581.487349	19.126144
51.943609	1582.407571	19.131162
51.666914	1596.829937	19.136179
51.982162	1594.250890	19.141197
51.791718	1598.589234	19.146215
51.485825	1587.107121	19.151232
51.856436	1600.323505	19.156250
51.741281	1616.109185	19.161267
52.159152	1624.173187	19.166285
52.378464	1621.742363	19.171303
52.515242	1623.764031	19.176320
52.472200	1620.121276	19.181338
52.236362	1626.783279	19.186355
51.957253	1625.172095	19.191373
52.955368	1622.893146	19.196391
52.584201	1627.856532	19.201408
52.668257	1622.385211	19.206426
52.521024	1635.088005	19.211443
52.850024	1630.135286	19.216461
53.124591	1644.896883	19.221479
53.061780	1652.747322	19.226496
53.179409	1644.402846	19.231514
52.877936	1649.601317	19.236531
53.010785	1645.269795	19.241549
53.098234	1646.965045	19.246567
53.042093	1653.323893	19.251584
53.186338	1645.262265	19.256602
52.973204	1640.905695	19.261619
53.227921	1640.209874	19.266637
53.181240	1639.618754	19.271655
53.169846	1647.095241	19.276672
53.392111	1647.575781	19.281690
53.173404	1649.200302	19.286707
53.398545	1641.632319	19.291725
53.708153	1648.835802	19.296743
53.423815	1646.528559	19.301760
53.769884	1650.174917	19.306778
53.708061	1672.526210	19.311795
53.941493	1665.933800	19.316813
54.204763	1662.127345	19.321831
54.091598	1656.434980	19.326848
54.026141	1641.221585	19.331866
53.859529	1643.902796	19.336883
54.008845	1640.466113	19.341901
53.709559	1658.345920	19.346919
54.042839	1669.063916	19.351936
54.270232	1675.314630	19.356954
54.143622	1681.379542	19.361971
54.133213	1666.441290	19.366989
54.182655	1665.423468	19.372007
54.396486	1673.762299	19.377024
54.433043	1670.116276	19.382042
54.370306	1672.931160	19.387059
54.163086	1665.763260	19.392077
54.509552	1663.888698	19.397095
54.658622	1684.208516	19.402112
54.874249	1688.596963	19.407130
54.634961	1699.250558	19.412147
54.853367	1690.813687	19.417165
55.191932	1686.144946	19.422183
54.710820	1690.315730	19.427200
55.345811	1686.929788	19.432218
55.167108	1691.930144	19.437235
54.979657	1694.188373	19.442253
55.210504	1686.593500	19.447271
54.927023	1686.674111	19.452288
55.461674	1680.259398	19.457306
55.080831	1687.565936	19.462323
55.119453	1686.943906	19.467341
55.546249	1682.732244	19.472359
55.345622	1687.724297	19.477376
55.537474	1680.141939	19.482394
55.299176	1686.831891	19.487411
55.459807	1687.175176	19.492429
55.239325	1690.253549	19.497447
55.209252	1714.954021	19.502464
55.832867	1709.117388	19.507482
55.525586	1723.106641	19.512499
55.739440	1721.568633	19.517517
56.110724	1721.478750	19.522535
55.919199	1722.523180	19.527552
55.713528	1709.312640	19.532570
56.017975	1718.191571	19.537587
55.938881	1716.252730	19.542605
56.251798	1708.607789	19.547623
56.470678	1716.685487	19.552640
56.566240	1713.476811	19.557658
56.591327	1713.672602	19.562675
56.464873	1720.728575	19.567693
56.511672	1710.178825	19.572711
56.406386	1708.543842	19.577728
56.640798	1709.089306	19.582746
56.609351	1716.180464	19.587763
56.666720	1710.537963	19.592781
56.583342	1713.859546	19.597799
56.651484	1718.966845	19.602816
56.647195	1724.291776	19.607834
56.819635	1743.664074	19.612851
56.680207	1742.071501	19.617869
56.928312	1739.099630	19.622887
56.682328	1742.663458	19.627904
56.906680	1741.222094	19.632922
57.275341	1730.341768	19.637939
56.580287	1741.147523	19.642957
56.945105	1739.782079	19.647975
56.843208	1758.855207	19.652992
57.472781	1761.231699	19.658010
57.202796	1776.546709	19.663027
57.142345	1769.743128	19.668045
57.649301	1767.153141	19.673063
57.383085	1773.064166	19.678080
57.558180	1766.263135	19.683098
57.374575	1771.303629	19.688115
57.564281	1773.131247	19.693133
57.604445	1776.327742	19.698151
57.902073	1795.544854	19.703168
58.149197	1790.369170	19.708186
58.471475	1800.545503	19.713203
58.780199	1770.956789	19.718221
58.771390	1743.747790	19.723239
58.701041	1750.709880	19.728256
58.788711	1745.923035	19.733274
59.034612	1733.988624	19.738291
58.865553	1720.677846	19.743309
58.947745	1706.960473	19.748327
58.780264	1713.411826	19.753344
58.822609	1712.074216	19.758362
59.372031	1706.683599	19.763379
59.105782	1710.179073	19.768397
59.178125	1686.772851	19.773415
58.862481	1688.806902	19.778432
58.683431	1679.559555	19.783450
59.026173	1678.421807	19.788467
58.736318	1675.841715	19.793485
58.939446	1673.334021	19.798503
58.552547	1675.033348	19.803520
58.743727	1680.783295	19.808538
59.053605	1693.750674	19.813555
59.082901	1701.107434	19.818573
58.998823	1695.643236	19.823591
58.753252	1708.420769	19.828608
58.801643	1697.921113	19.833626
59.283068	1698.334368	19.838643
58.819593	1704.066026	19.843661
58.987832	1715.039269	19.848679
59.153016	1734.334056	19.853696
59.389680	1733.935286	19.858714
59.483890	1740.160074	19.863731
59.326031	1744.339098	19.868749
59.510401	1735.794364	19.873767
59.432933	1740.004614	19.878784
59.466648	1757.896719	19.883802
60.032437	1767.093462	19.888819
59.938208	1773.316067	19.893837
60.352616	1757.130123	19.898855
60.019584	1768.276950	19.903872
60.331864	1765.302705	19.908890
60.393879	1761.237293	19.913907
60.138328	1768.210837	19.918925
60.395947	1758.216567	19.923943
60.227707	1768.276037	19.928960
60.174004	1763.553420	19.933978
60.284733	1768.134025	19.938995
60.279852	1765.740506	19.944013
60.361907	1763.309525	19.949031
60.494662	1787.437490	19.954048
60.817251	1779.920753	19.959066
60.950980	1784.113851	19.964083
60.511479	1791.661833	19.969101
60.860146	1786.477035	19.974119
60.701457	1791.910778	19.979136
60.961954	1783.710189	19.984154
60.716629	1785.034569	19.989171
60.823723	1790.200179	19.994189
60.881275	1778.129805	19.999207
60.954485	1800.175810	20.004224
60.971784	1802.328250	20.009242
61.422369	1808.866706	20.014259
61.270390	1816.438850	20.019277
61.435841	1811.951059	20.024295
61.658551	1814.240641	20.029312
61.373271	1813.334396	20.034330
61.429377	1814.530476	20.039347
61.202076	1823.003458	20.044365
61.698323	1829.278219	20.049383
61.758659	1844.986606	20.054400
61.694247	1846.642387	20.059418
61.866760	1841.301606	20.064435
61.577353	1849.109631	20.069453
62.072226	1832.854138	20.074471
62.119563	1835.029322	20.079488
62.110703	1839.895669	20.084506
62.281234	1835.095579	20.089523
62.281924	1837.799698	20.094541
62.254989	1835.592169	20.099559
62.205798	1847.414285	20.104576
62.549286	1856.235949	20.109594
62.612454	1860.271210	20.114611
62.492482	1866.112541	20.119629
62.709626	1865.760929	20.124647
62.799292	1861.645458	20.129664
62.606616	1865.649944	20.134682
62.492943	1870.562120	20.139699
62.451664	1870.396450	20.144717
63.199842	1864.178070	20.149735
62.869349	1870.237034	20.154752
62.665830	1870.978984	20.159770
63.056184	1866.637006	20.164787
62.677203	1869.859465	20.169805
63.024995	1875.854307	20.174823
63.115625	1893.661992	20.179840
62.988360	1904.399338	20.184858
63.481159	1899.909655	20.189875
63.412979	1902.351043	20.194893
63.590522	1890.621690	20.199911
63.256543	1898.268523	20.204928
63.661003	1894.708500	20.209946
63.630576	1883.023333	20.214963
63.702033	1894.190697	20.219981
64.076764	1904.910125	20.224999
64.246816	1913.148316	20.230016
63.970867	1904.249787	20.235034
64.131897	1899.079929	20.240051
64.192649	1910.468467	20.245069
64.455121	1910.363688	20.250087
64.127364	1902.425961	20.255104
64.206443	1915.583728	20.260122
64.561661	1907.871371	20.265139
64.366066	1912.603129	20.270157
64.718724	1905.078386	20.275175
64.508916	1905.498846	20.280192
64.602579	1906.405777	20.285210
64.795791	1901.707450	20.290227
64.537931	1912.165945	20.295245
64.754028	1903.560993	20.300263
64.427464	1909.814417	20.305280
64.543272	1905.473738	20.310298
64.726454	1899.972347	20.315315
64.454920	1913.919112	20.320333
64.913250	1934.587965	20.325351
65.167396	1933.561076	20.330368
65.185664	1928.092268	20.335386
65.177353	1934.588339	20.340403
64.940178	1935.857945	20.345421
65.267989	1938.907920	20.350439
65.490674	1932.628587	20.355456
65.235737	1932.504070	20.360474
65.606222	1939.817550	20.365491
65.590853	1950.853289	20.370509
65.557450	1955.982371	20.375527
65.952287	1955.938287	20.380544
65.951965	1960.175625	20.385562
65.819993	1960.809420	20.390579
65.563120	1961.155583	20.395597
65.719587	1964.134567	20.400615
65.746806	1953.718335	20.405632
65.814010	1954.101698	20.410650
66.343619	1950.468216	20.415667
66.086433	1953.749140	20.420685
66.135801	1957.772470	20.425703
66.313999	1964.748512	20.430720
66.444973	1979.276926	20.435738
66.482084	1983.411553	20.440755
66.463421	1988.361316	20.445773
66.763151	1979.810628	20.450791
66.715563	1980.586708	20.455808
66.466411	1990.153466	20.460826
66.881615	1980.177962	20.465843
66.687043	1984.583937	20.470861
66.460006	1990.182035	20.475879
66.779277	1986.484554	20.480896
66.828968	1999.864965	20.485914
67.113706	2005.414488	20.490931
66.929922	2014.398208	20.495949
67.013503	2008.430488	20.500967
67.283371	2009.435178	20.505984
67.359226	2015.172973	20.511002
67.544782	2004.849440	20.516019
67.584870	2009.395766	20.521037
67.208191	2004.187345	20.526055
67.531268	2020.571378	20.531072
67.663178	2032.452860	20.536090
67.925029	2032.068158	20.541107
67.879161	2036.391440	20.546125
68.168581	2028.697379	20.551143
68.809242	2026.663376	20.556160
68.645920	2021.871633	20.561178
68.421430	2003.912890	20.566195
68.238774	1997.647045	20.571213
68.059413	1993.771872	20.576231
68.344611	1987.552552	20.581248
68.467435	1992.280749	20.586266
68.495358	2009.105916	20.591283
68.501440	2019.638808	20.596301
68.321625	2022.606149	20.601319
68.425080	2017.295982	20.606336
68.709525	2024.525691	20.611354
68.840699	2019.064013	20.616371
68.646855	2017.439971	20.621389
68.668115	2016.052995	20.626407
68.772760	2024.940383	20.631424
68.486467	2029.238292	20.636442
68.991045	2031.548243	20.641459
69.052342	2045.806241	20.646477
68.984968	2045.791034	20.651495
69.011814	2044.555761	20.656512
69.113716	2053.908473	20.661530
69.177891	2045.344971	20.666547
69.154238	2045.546967	20.671565
69.171406	2063.899091	20.676583
69.595337	2075.173204	20.681600
69.459521	2080.395748	20.686618
69.944223	2078.365372	20.691635
69.570221	2083.858731	20.696653
69.507463	2086.695721	20.701671
70.072620	2073.532608	20.706688
70.208247	2065.017480	20.711706
70.568214	2064.903445	20.716723
70.659022	2066.450333	20.721741
70.497008	2071.980672	20.726759
70.598879	2065.380747	20.731776
70.356471	2064.719354	20.736794
70.573046	2067.711586	20.741811
70.535975	2068.551280	20.746829
70.673300	2071.003184	20.751847
70.729629	2066.944100	20.756864
70.515295	2071.745756	20.761882
70.652543	2068.159874	20.766899
70.531844	2066.476967	20.771917
70.309917	2072.937161	20.776935
70.748678	2080.209934	20.781952
70.919826	2092.953595	20.786970
70.768735	2085.626298	20.791987
70.966008	2095.710293	20.797005
70.705542	2101.486026	20.802023
70.949632	2107.097132	20.807040
71.162267	2135.752308	20.812058
71.300978	2131.182160	20.817075
71.569368	2129.516640	20.822093
71.302651	2136.145254	20.827111
71.601086	2133.265175	20.832128
71.420497	2127.551914	20.837146
71.617886	2137.462084	20.842163
71.882104	2147.041464	20.847181
71.897720	2160.360596	20.852199
72.504380	2149.562354	20.857216
72.314319	2152.045244	20.862234
72.327040	2148.828446	20.867251
72.768458	2148.393080	20.872269
72.184611	2143.199556	20.877287
72.685811	2140.802352	20.882304
72.675440	2149.186652	20.887322
72.821876	2139.068269	20.892339
72.586477	2120.396116	20.897357
72.472883	2123.946000	20.902375
72.854040	2129.890006	20.907392
72.776384	2141.758590	20.912410
72.827262	2139.805257	20.917427
73.097354	2144.180438	20.922445
72.918725	2144.110608	20.927463
73.000705	2139.342633	20.932480
72.941213	2148.306613	20.937498
73.092603	2142.990330	20.942515
73.297837	2136.093865	20.947533
73.002179	2143.490085	20.952551
73.249758	2137.666848	20.957568
73.371757	2141.189390	20.962586
73.298096	2145.774350	20.967603
73.510069	2147.130448	20.972621
73.413055	2164.943219	20.977639
73.635881	2170.778771	20.982656
73.607964	2177.440901	20.987674
73.817143	2180.570415	20.992691
73.609389	2172.933543	20.997709
73.517066	2183.637991	21.002727
73.884228	2178.791487	21.007744
74.005189	2192.502087	21.012762
73.829714	2209.806704	21.017779
73.832931	2206.220139	21.022797
73.747244	2205.639149	21.027815
74.076925	2212.041326	21.032832
73.966377	2231.897535	21.037850
74.203088	2236.391337	21.042867
74.539749	2242.067178	21.047885
74.451677	2241.406335	21.052903
74.645017	2236.534830	21.057920
75.071342	2247.902302	21.062938
75.683222	2242.754816	21.067955
75.495572	2235.423834	21.072973
75.581320	2217.564804	21.077991
75.606509	2206.533603	21.083008
75.626988	2211.255382	21.088026
75.962852	2198.450438	21.093043
76.375174	2190.423632	21.098061
76.193082	2186.977533	21.103079
76.105607	2165.718242	21.108096
76.157943	2162.788520	21.113114
76.199145	2168.114225	21.118131
76.216076	2160.980338	21.123149
76.063739	2166.607493	21.128167
76.236675	2160.653778	21.133184
76.096970	2163.142798	21.138202
75.883371	2163.124953	21.143219
76.401241	2146.569690	21.148237
76.072218	2163.889301	21.153255
76.241366	2151.365839	21.158272
76.073603	2158.212299	21.163290
76.169486	2152.074229	21.168307
76.311599	2146.050710	21.173325
76.446643	2160.583378	21.178343
76.577658	2166.449302	21.183360
76.586847	2190.739228	21.188378
76.523417	2189.666218	21.193395
76.851174	2186.686275	21.198413
76.400310	2192.910872	21.203431
76.812989	2196.652939	21.208448
77.215560	2196.018469	21.213466
76.700156	2191.715441	21.218483
77.060057	2199.112547	21.223501
76.881043	2209.465862	21.228519
76.770126	2215.106881	21.233536
77.178393	2219.381392	21.238554
77.256320	2224.450338	21.243571
77.743616	2209.916696	21.248589
77.303843	2221.486768	21.253607
77.703950	2229.510683	21.258624
77.865213	2235.091785	21.263642
77.716333	2245.326265	21.268659
77.795746	2235.835977	21.273677
77.888544	2247.913441	21.278695
78.166071	2237.346966	21.283712
78.052073	2236.578562	21.288730
78.078333	2237.464800	21.293747
78.497017	2232.116084	21.298765
78.296562	2233.102977	21.303783
78.589164	2232.929680	21.308800
78.895302	2233.173477	21.313818
78.983369	2229.035347	21.318835
78.668572	2232.177640	21.323853
78.695580	2243.008621	21.328871
78.860940	2239.921632	21.333888
78.775933	2248.152708	21.338906
78.679443	2250.396513	21.343923
78.917697	2259.949432	21.348941
78.816837	2260.197567	21.353959
78.563201	2251.908018	21.358976
79.225511	2258.998141	21.363994
79.301328	2275.882051	21.369011
79.564931	2277.800208	21.374029
79.524949	2285.508906	21.379047
79.530399	2276.076796	21.384064
79.435690	2280.544020	21.389082
79.552468	2282.139491	21.394099
79.908468	2265.919826	21.399117
79.621036	2289.138684	21.404135
79.653692	2303.721646	21.409152
80.225353	2304.155932	21.414170
79.750090	2312.866960	21.419187
80.022260	2303.036758	21.424205
80.004790	2309.868760	21.429223
80.294080	2319.644051	21.434240
80.460260	2331.318157	21.439258
80.301486	2338.075955	21.444275
80.923731	2339.416986	21.449293
80.716126	2342.614575	21.454311
80.610747	2342.323040	21.459328
80.991226	2341.945372	21.464346
80.727786	2338.657729	21.469363
81.003100	2343.761314	21.474381
80.836337	2345.390997	21.479399
81.026913	2341.028040	21.484416
81.373353	2331.912789	21.489434
81.069720	2350.133942	21.494451
81.205464	2351.305567	21.499469
81.585477	2356.560005	21.504487
81.668762	2362.131567	21.509504
81.952121	2361.203823	21.514522
81.789615	2367.458807	21.519539
82.039381	2364.501493	21.524557
81.890554	2370.955666	21.529575
81.783538	2368.219647	21.534592
82.273917	2363.808874	21.539610
82.217049	2366.328767	21.544627
82.217592	2355.715920	21.549645
82.050408	2362.902978	21.554663
82.160376	2364.973863	21.559680
82.208124	2362.844802	21.564698
82.077784	2369.598866	21.569715
82.400627	2383.931902	21.574733
82.573866	2394.762487	21.579751
82.814558	2401.863282	21.584768
82.667616	2400.536917	21.589786
82.223819	2408.333675	21.594803
83.072211	2404.304719	21.599821
83.210679	2414.892298	21.604839
83.137346	2425.125081	21.609856
83.168335	2425.003729	21.614874
83.264321	2426.103040	21.619891
83.047049	2423.017251	21.624909
83.159678	2427.210755	21.629927
83.250852	2424.524139	21.634944
83.535905	2424.727253	21.639962
83.502739	2445.494094	21.644979
83.698982	2451.014639	21.649997
83.693902	2451.382012	21.655015
83.783900	2459.092884	21.660032
83.807115	2460.903093	21.665050
83.739058	2463.142397	21.670067
83.811213	2457.268349	21.675085
84.059534	2473.738757	21.680103
84.443639	2480.191370	21.685120
84.968438	2477.805298	21.690138
84.508958	2490.887429	21.695155
84.815255	2479.832430	21.700173
84.891887	2472.099706	21.705191
85.189238	2478.293989	21.710208
84.789056	2471.691350	21.715226
84.852457	2470.465944	21.720243
85.317104	2460.747318	21.725261
85.133323	2475.844007	21.730279
85.065802	2474.808599	21.735296
85.881919	2454.470638	21.740314
85.837992	2457.076583	21.745331
85.640389	2458.647481	21.750349
86.200520	2453.202975	21.755367
86.142413	2453.904457	21.760384
85.994213	2432.321729	21.765402
85.726731	2431.450360	21.770419
86.069627	2426.492016	21.775437
85.944171	2424.610028	21.780455
86.122415	2434.019245	21.785472
86.343251	2431.825601	21.790490
86.283805	2441.940551	21.795507
86.552517	2436.139784	21.800525
86.366034	2427.016642	21.805543
86.207603	2438.168382	21.810560
86.498711	2440.285905	21.815578
86.561612	2441.049109	21.820595
86.484842	2438.023503	21.825613
86.195336	2447.133685	21.830631
86.094898	2441.809470	21.835648
86.575474	2458.431608	21.840666
86.495082	2470.741392	21.845683
86.710143	2474.835982	21.850701
87.031408	2478.037360	21.855719
86.845580	2491.309472	21.860736
87.250257	2502.301454	21.865754
87.410485	2509.467836	21.870771
87.307630	2501.650448	21.875789
87.557469	2497.367667	21.880807
87.470228	2510.206388	21.885824
87.898203	2504.366825	21.890842
87.164400	2505.939856	21.895859
87.661952	2523.926481	21.900877
88.007892	2529.135287	21.905895
87.838021	2537.922029	21.910912
88.297076	2531.768363	21.915930
88.276016	2537.884445	21.920947
88.370353	2534.102349	21.925965
87.897530	2534.149438	21.930983
88.273508	2552.932653	21.936000
88.712534	2556.201010	21.941018
88.551787	2557.317675	21.946035
88.958239	2560.705285	21.951053
89.122221	2558.493158	21.956071
89.043700	2553.196085	21.961088
89.039133	2555.247505	21.966106
88.981304	2549.372124	21.971123
89.123639	2550.416071	21.976141
89.480592	2552.485353	21.981159
89.137416	2567.815220	21.986176
89.534501	2571.857212	21.991194
89.723398	2587.289463	21.996211
89.612596	2586.587391	22.001229
89.909572	2584.748143	22.006247
89.854972	2589.982301	22.011264
89.627914	2584.473707	22.016282
89.567309	2590.188654	22.021299
89.257884	2585.152575	22.026317
89.657753	2598.518597	22.031335
89.753733	2609.482014	22.036352
90.044800	2607.979588	22.041370
89.782719	2609.991060	22.046387
90.043759	2626.904048	22.051405
90.457202	2636.939002	22.056423
90.062181	2639.726039	22.061440
90.601524	2643.649398	22.066458
90.321674	2638.113805	22.071475
90.547067	2657.338073	22.076493
91.061968	2656.444184	22.081511
91.063456	2661.632452	22.086528
91.491498	2656.938914	22.091546
91.357399	2657.064138	22.096563
91.349198	2664.622444	22.101581
91.727144	2655.820548	22.106599
91.624377	2661.406162	22.111616
91.375632	2650.591364	22.116634
91.762405	2661.651612	22.121651
91.996592	2677.402393	22.126669
92.013998	2681.860512	22.131687
92.145716	2685.457153	22.136704
92.318558	2680.905777	22.141722
92.694294	2681.611241	22.146739
92.759989	2675.684646	22.151757
93.237349	2657.824772	22.156775
93.077439	2646.584411	22.161792
93.240234	2633.869618	22.166810
92.915789	2634.346133	22.171827
92.829680	2635.616089	22.176845
93.146891	2630.211045	22.181863
92.811787	2629.603736	22.186880
92.888388	2630.540966	22.191898
93.017316	2629.747960	22.196915
93.025511	2642.008364	22.201933
93.194603	2638.216680	22.206951
93.063849	2649.275279	22.211968
93.204502	2656.568354	22.216986
92.950198	2671.405896	22.222003
93.528323	2664.595244	22.227021
93.265657	2674.867833	22.232039
93.304092	2694.241529	22.237056
93.644770	2688.980604	22.242074
93.923856	2697.028799	22.247091
93.603656	2699.685922	22.252109
93.752523	2709.306881	22.257127
94.070420	2725.023914	22.262144
94.162358	2727.344724	22.267162
94.223631	2730.582113	22.272179
94.266196	2720.309984	22.277197
94.771200	2738.125778	22.282215
94.393494	2755.282365	22.287232
94.726438	2753.126647	22.292250
95.072597	2762.956099	22.297267
94.997171	2754.194191	22.302285
95.337395	2753.320286	22.307303
95.173545	2750.509877	22.312320
95.268839	2748.977300	22.317338
95.396422	2758.843964	22.322355
95.390695	2750.343114	22.327373
95.372181	2742.751278	22.332391
95.370168	2754.474571	22.337408
95.481560	2760.559399	22.342426
95.898766	2779.691884	22.347443
95.444916	2792.804848	22.352461
95.765564	2783.431488	22.357479
95.683763	2786.790820	22.362496
95.946846	2789.546880	22.367514
96.320171	2797.613927	22.372531
96.138674	2809.226653	22.377549
96.279938	2809.444838	22.382567
96.166437	2811.592327	22.387584
96.471297	2811.371448	22.392602
96.451514	2820.475033	22.397619
96.787894	2827.894306	22.402637
96.864528	2837.402581	22.407655
97.357528	2840.184131	22.412672
97.056621	2844.373691	22.417690
96.976469	2845.232098	22.422707
97.101307	2843.255078	22.427725
97.367634	2838.639189	22.432743
97.515005	2852.995164	22.437760
97.340488	2863.879194	22.442778
97.889441	2855.748432	22.447795
97.757795	2866.920611	22.452813
97.804759	2863.525925	22.457831
97.371310	2871.569847	22.462848
97.855812	2869.996432	22.467866
98.177423	2883.794467	22.472883
98.077577	2894.794832	22.477901
98.605975	2885.805977	22.482919
98.476454	2898.681672	22.487936
98.608754	2897.711910	22.492954
98.877941	2889.997030	22.497971
98.709451	2899.133816	22.502989
99.082672	2885.211604	22.508007
98.715348	2895.235157	22.513024
98.796346	2882.130440	22.518042
98.964063	2897.668659	22.523059
99.016372	2915.721264	22.528077
99.274789	2910.784883	22.533095
99.234642	2927.352936	22.538112
99.033240	2917.416919	22.543130
99.346664	2922.695557	22.548147
99.632957	2938.307732	22.553165
99.495484	2952.150721	22.558183
99.807853	2954.106818	22.563200
99.859946	2947.866845	22.568218
100.048587	2953.863131	22.573235
99.702098	2955.705611	22.578253
100.283981	2965.404001	22.583271
100.405180	2976.332207	22.588288
100.398820	2979.869916	22.593306
100.676926	2972.189756	22.598323
100.608512	2972.494084	22.603341
101.060942	2970.290177	22.608359
101.085683	2968.560372	22.613376
101.341544	2961.347877	22.618394
101.129002	2963.360935	22.623411
101.170670	2971.686277	22.628429
101.566758	2955.133796	22.633447
101.619427	2957.870738	22.638464
101.359107	2958.410192	22.643482
101.654078	2951.031779	22.648499
101.762524	2960.357284	22.653517
101.592227	2957.452680	22.658535
101.886290	2967.454196	22.663552
101.894144	2988.850077	22.668570
102.182338	2983.124654	22.673587
102.040242	2987.963858	22.678605
102.013419	2979.419041	22.683623
101.905219	2987.068190	22.688640
101.801179	2997.032521	22.693658
102.464052	3010.833682	22.698675
102.303160	3025.685790	22.703693
102.458228	3019.770764	22.708711
102.590983	3014.424887	22.713728
102.932554	3030.006319	22.718746
103.298993	3037.457092	22.723763
103.562423	3045.866682	22.728781
103.706522	3036.876086	22.733799
104.052833	3037.894623	22.738816
103.331284	3020.765122	22.743834
103.840516	3018.687452	22.748851
103.828824	3032.766115	22.753869
103.915387	3029.699394	22.758887
104.107630	3031.478000	22.763904
104.218438	3023.685258	22.768922
104.237305	3023.471438	22.773939
104.293801	3027.796781	22.778957
104.426236	3022.937877	22.783975
104.257791	3019.685273	22.788992
104.441971	3026.295088	22.794010
104.559124	3019.968405	22.799027
104.680181	3027.426051	22.804045
104.974635	3029.459746	22.809063
104.868697	3025.060489	22.814080
104.731806	3025.702977	22.819098
105.069689	3034.570308	22.824115
104.981851	3050.760655	22.829133
104.780974	3054.788008	22.834151
105.314103	3048.519269	22.839168
105.428151	3053.054913	22.844186
105.489182	3056.665278	22.849203
105.321595	3070.576898	22.854221
105.712287	3080.686586	22.859239
105.736338	3078.772806	22.864256
105.328225	3075.473450	22.869274
105.921849	3067.420407	22.874291
105.886620	3085.152861	22.879309
106.090953	3096.933200	22.884327
106.540157	3100.874995	22.889344
106.612676	3108.010821	22.894362
106.774590	3099.116463	22.899379
106.921845	3098.892395	22.904397
106.830451	3100.770517	22.909415
106.999314	3097.353192	22.914432
106.786544	3102.159651	22.919450
106.999073	3100.292903	22.924467
106.998154	3117.746175	22.929485
107.229961	3123.604281	22.934503
107.257536	3122.508036	22.939520
107.449481	3128.439365	22.944538
107.458804	3121.756967	22.949555
107.296704	3126.118770	22.954573
107.535323	3138.892706	22.959591
107.808973	3151.528125	22.964608
107.747479	3161.041332	22.969626
108.323195	3148.127307	22.974643
108.050645	3156.096954	22.979661
107.927963	3179.526153	22.984679
108.338036	3178.749645	22.989696
108.553861	3180.511137	22.994714
108.724249	3182.172891	22.999731
108.622919	3183.099199	23.004749
109.049611	3179.305632	23.009767
108.986362	3197.631097	23.014784
108.880249	3214.422387	23.019802
109.319024	3209.558624	23.024819
109.408477	3211.967225	23.029837
108.898556	3223.787618	23.034855
109.102031	3214.715075	23.039872
109.441250	3238.812518	23.044890
109.631429	3248.655372	23.049907
109.876547	3244.200855	23.054925
109.622098	3241.976687	23.059943
109.896881	3238.128664	23.064960
109.684362	3272.095279	23.069978
110.282576	3264.503946	23.074995
110.435907	3273.546381	23.080013
110.098790	3279.614054	23.085031
110.527760	3279.763557	23.090048
110.364608	3298.025627	23.095066
110.666923	3302.941957	23.100083
110.910529	3295.858690	23.105101
111.282891	3300.524710	23.110119
111.209711	3304.348479	23.115136
110.900841	3304.551134	23.120154
111.202286	3316.943123	23.125171
111.477468	3326.037745	23.130189
111.600267	3324.709186	23.135207
112.017843	3322.431336	23.140224
111.897885	3325.723716	23.145242
112.044877	3322.212282	23.150259
111.795417	3328.425687	23.155277
112.291784	3320.035598	23.160295
112.288481	3316.478907	23.165312
112.041302	3320.467303	23.170330
112.306313	3315.428260	23.175347
112.607705	3346.373394	23.180365
112.489739	3349.108513	23.185383
112.719755	3342.921812	23.190400
113.119105	3344.871174	23.195418
113.170678	3352.968599	23.200435
112.928362	3355.743214	23.205453
113.049044	3351.468198	23.210471
113.168523	3351.478258	23.215488
113.108256	3372.671593	23.220506
113.385513	3363.854655	23.225523
113.757660	3366.395200	23.230541
113.424626	3368.726452	23.235559
114.040302	3365.482466	23.240576
114.000632	3382.554413	23.245594
114.015377	3394.742030	23.250611
114.264078	3388.566491	23.255629
114.210545	3388.475128	23.260647
114.430997	3386.933542	23.265664
114.191814	3392.343736	23.270682
114.299935	3398.485204	23.275699
114.500752	3415.613241	23.280717
114.813128	3423.767448	23.285735
115.050705	3419.674370	23.290752
115.167676	3423.486728	23.295770
115.410101	3419.436142	23.300787
115.511908	3420.370192	23.305805
115.850262	3438.415589	23.310823
115.963166	3437.311221	23.315840
115.657312	3439.083559	23.320858
116.171081	3440.052611	23.325875
116.193993	3446.023609	23.330893
116.058655	3457.837950	23.335911
116.322188	3441.507445	23.340928
116.180115	3446.290156	23.345946
116.480730	3447.645620	23.350963
116.296258	3442.796992	23.355981
116.269163	3439.583113	23.360999
116.442813	3444.936937	23.366016
116.815025	3460.934806	23.371034
116.718592	3456.894190	23.376051
117.175995	3458.318266	23.381069
117.241743	3458.484785	23.386087
117.225163	3460.269211	23.391104
117.382174	3463.749520	23.396122
117.277372	3469.925757	23.401139
117.534736	3485.106537	23.406157
117.317392	3493.124201	23.411175
117.645699	3487.002006	23.416192
117.861451	3496.283996	23.421210
117.922250	3489.174721	23.426227
118.509538	3498.194510	23.431245
118.241993	3508.398444	23.436263
118.350319	3510.540555	23.441280
118.370987	3516.218516	23.446298
118.402611	3511.451832	23.451315
118.610569	3507.920407	23.456333
118.805008	3515.024403	23.461351
118.961386	3524.389825	23.466368
119.181611	3540.441123	23.471386
119.138578	3546.600463	23.476403
119.453898	3535.536944	23.481421
119.221173	3542.230778	23.486439
119.404678	3540.045287	23.491456
119.731480	3541.135413	23.496474
119.492476	3546.260863	23.501491
119.877698	3554.871593	23.506509
119.793875	3567.428282	23.511527
119.796862	3571.576666	23.516544
119.959428	3581.419428	23.521562
120.359964	3604.997941	23.526579
120.438297	3602.106267	23.531597
120.325743	3611.405281	23.536615
120.549392	3598.879763	23.541632
120.512342	3603.359433	23.546650
120.848041	3626.680854	23.551667
120.881071	3628.403109	23.556685
120.819988	3628.666948	23.561703
121.320057	3624.567357	23.566720
121.450912	3640.597615	23.571738
121.207194	3659.015366	23.576755
121.626773	3663.598455	23.581773
121.216875	3662.929074	23.586791
121.462857	3665.817832	23.591808
121.638341	3686.872548	23.596826
121.625590	3692.704586	23.601843
122.051207	3706.609537	23.606861
122.187617	3726.536163	23.611879
122.444901	3720.921586	23.616896
122.407290	3727.482125	23.621914
122.437734	3729.431365	23.626931
122.952569	3737.444119	23.631949
122.950908	3746.174866	23.636967
122.990722	3754.858098	23.641984
123.142591	3745.205814	23.647002
122.949744	3753.032485	23.652019
123.509988	3756.273926	23.657037
123.432102	3773.374447	23.662055
123.985007	3786.507119	23.667072
123.844418	3781.641154	23.672090
123.925237	3781.141322	23.677107
124.227612	3781.088393	23.682125
123.679578	3779.156396	23.687143
124.355133	3780.067423	23.692160
124.855826	3782.431785	23.697178
125.215297	3793.145606	23.702195
125.249307	3771.223472	23.707213
125.164272	3759.753980	23.712231
125.258907	3767.871514	23.717248
125.235922	3755.965755	23.722266
125.158745	3760.909714	23.727283
125.859555	3774.050258	23.732301
125.634284	3769.432228	23.737319
125.848746	3779.458010	23.742336
125.514846	3784.287938	23.747354
125.617858	3788.333113	23.752371
125.993928	3792.369363	23.757389
125.836127	3798.803564	23.762407
125.829938	3786.073814	23.767424
126.206341	3801.920348	23.772442
126.083569	3820.538497	23.777459
126.572655	3814.641480	23.782477
126.563502	3824.872084	23.787495
126.434571	3826.963965	23.792512
126.469322	3844.550869	23.797530
126.501459	3851.323758	23.802547
126.787356	3850.390018	23.807565
126.956172	3875.402267	23.812583
127.193994	3873.432269	23.817600
127.645335	3875.478832	23.822618
127.464905	3882.950373	23.827635
127.674376	3877.149051	23.832653
127.868791	3878.150966	23.837671
128.122201	3894.431004	23.842688
127.977018	3898.981500	23.847706
128.213244	3898.201213	23.852723
128.415290	3885.180930	23.857741
127.932095	3899.492942	23.862759
128.125178	3916.060322	23.867776
128.754320	3925.762837	23.872794
128.675839	3925.292335	23.877811
129.228939	3930.774637	23.882829
129.121747	3945.484587	23.887847
129.336223	3946.879009	23.892864
129.558961	3955.456884	23.897882
129.431167	3954.589889	23.902899
129.846570	3956.919893	23.907917
129.649524	3953.854935	23.912935
129.726211	3952.233161	23.917952
130.123209	3960.286856	23.922970
130.271268	3981.047428	23.927987
130.468876	3968.598911	23.933005
130.453377	3976.132309	23.938023
131.030846	3971.792932	23.943040
131.196431	3978.313316	23.948058
131.159329	3976.712830	23.953075
131.537505	3964.037281	23.958093
131.364738	3963.584958	23.963111
131.592173	3961.357001	23.968128
131.909820	3952.969095	23.973146
131.630206	3953.097860	23.978163
131.634419	3948.003427	23.983181
131.514434	3948.846221	23.988199
131.975898	3951.585035	23.993216
132.051594	3952.697140	23.998234
131.675894	3951.880688	24.003251
132.304006	3957.011979	24.008269
132.287960	3973.992738	24.013287
132.281053	3975.895260	24.018304
132.389849	3969.954191	24.023322
132.133694	3982.561526	24.028339
132.419301	3993.167697	24.033357
132.746263	4011.302941	24.038375
133.015802	4008.084119	24.043392
132.987503	4005.457962	24.048410
133.211258	4026.049191	24.053427
133.311703	4027.836266	24.058445
133.161285	4041.542313	24.063463
133.420556	4047.725248	24.068480
133.927254	4053.355813	24.073498
134.085165	4059.196972	24.078515
134.069060	4065.184670	24.083533
134.446813	4063.012971	24.088551
134.359770	4054.576253	24.093568
134.911782	4061.743864	24.098586
134.744041	4078.297373	24.103603
135.189655	4074.282653	24.108621
135.107378	4083.251448	24.113639
135.146175	4088.556995	24.118656
135.245086	4085.281975	24.123674
135.173274	4090.708216	24.128691
135.203160	4086.119416	24.133709
135.701872	4100.165706	24.138727
135.893829	4108.605402	24.143744
136.199461	4107.354611	24.148762
136.286921	4107.885848	24.153779
136.246765	4099.827106	24.158797
136.733442	4106.256229	24.163815
136.263216	4100.873153	24.168832
136.792498	4100.625134	24.173850
137.094765	4111.863594	24.178867
137.162227	4115.605359	24.183885
137.369450	4128.008342	24.188903
137.205492	4127.743415	24.193920
137.233545	4118.542524	24.198938
137.324131	4127.884209	24.203955
137.863016	4130.333011	24.208973
137.876388	4129.830549	24.213991
137.660124	4130.006643	24.219008
138.086840	4117.697688	24.224026
138.103571	4125.652411	24.229043
138.380974	4140.088039	24.234061
138.687640	4144.668046	24.239079
138.731719	4146.896018	24.244096
138.916755	4146.126242	24.249114
138.568578	4157.761887	24.254131
138.570767	4150.806389	24.259149
138.583513	4147.559254	24.264167
138.742241	4146.013274	24.269184
139.051369	4156.715724	24.274202
139.092380	4167.287860	24.279219
139.093119	4174.843945	24.284237
139.191508	4176.058653	24.289255
139.252504	4200.681927	24.294272
139.688558	4198.862008	24.299290
139.603678	4210.538314	24.304307
139.635186	4231.815804	24.309325
140.012173	4243.143148	24.314343
140.002547	4245.470168	24.319360
141.029927	4236.799797	24.324378
141.440691	4251.139535	24.329395
141.678220	4243.495082	24.334413
141.111292	4234.368533	24.339431
141.525383	4244.900119	24.344448
141.722454	4250.529782	24.349466
141.572329	4250.232753	24.354483
141.764011	4248.019108	24.359501
141.736519	4242.934347	24.364519
141.562378	4249.470473	24.369536
141.982904	4244.096362	24.374554
141.972960	4253.061593	24.379571
142.398805	4259.334490	24.384589
142.342608	4260.798063	24.389607
142.284492	4272.560621	24.394624
142.437945	4261.772541	24.399642
142.346001	4286.613873	24.404659
142.778043	4292.117977	24.409677
143.112294	4294.323305	24.414695
142.771164	4307.580120	24.419712
143.118661	4316.807798	24.424730
143.096721	4325.476826	24.429747
143.120916	4340.595761	24.434765
143.338718	4355.457271	24.439783
143.665890	4370.854410	24.444800
144.367949	4366.243312	24.449818
144.807910	4375.768606	24.454835
145.266246	4369.770857	24.459853
145.377300	4343.183015	24.464871
145.222977	4339.388183	24.469888
145.638073	4339.794812	24.474906
145.461288	4330.625662	24.479923
145.784316	4328.911074	24.484941
146.001897	4323.178302	24.489959
145.859517	4323.452754	24.494976
146.078550	4317.983298	24.499994
145.986232	4327.378661	24.505011
145.991250	4322.295770	24.510029
146.441492	4312.556993	24.515047
146.263915	4316.900372	24.520064
146.511779	4315.775996	24.525082
146.378942	4313.906738	24.530099
146.026558	4317.108163	24.535117
146.386578	4317.227774	24.540135
146.193988	4332.002075	24.545152
146.842259	4343.639474	24.550170
146.758737	4348.328176	24.555187
146.727759	4364.533717	24.560205
147.361543	4371.031547	24.565223
147.503655	4376.204294	24.570240
147.586300	4370.496952	24.575258
147.462230	4389.822488	24.580275
147.665617	4403.137322	24.585293
147.942546	4401.083138	24.590311
148.091658	4412.891437	24.595328
148.268835	4422.817401	24.600346
148.006428	4448.546844	24.605363
148.068912	4448.756379	24.610381
148.418111	4448.037511	24.615399
148.809389	4468.538928	24.620416
149.091461	4464.852279	24.625434
149.279847	4468.880885	24.630451
149.239136	4497.369459	24.635469
149.702197	4489.161037	24.640487
149.690526	4495.817695	24.645504
150.007549	4484.744543	24.650522
150.321143	4494.876951	24.655539
150.117667	4501.508337	24.660557
151.029522	4504.199836	24.665575
150.656455	4522.711664	24.670592
150.366340	4516.524802	24.675610
150.692243	4520.324590	24.680627
150.781477	4521.876714	24.685645
150.966049	4527.993093	24.690663
150.966740	4546.707333	24.695680
151.327359	4554.559467	24.700698
151.218565	4550.735293	24.705715
151.272021	4552.310432	24.710733
151.555754	4574.441909	24.715751
151.537270	4569.251753	24.720768
151.784796	4590.824167	24.725786
152.054894	4602.825742	24.730803
152.124487	4611.972042	24.735821
152.473670	4603.905230	24.740839
152.534741	4633.351794	24.745856
152.768513	4641.282416	24.750874
153.004929	4647.671438	24.755891
152.881606	4651.080295	24.760909
153.235771	4656.403423	24.765927
153.109660	4673.888731	24.770944
153.234396	4669.684280	24.775962
153.509103	4683.329433	24.780979
153.604858	4681.162489	24.785997
153.561333	4684.357230	24.791015
153.829768	4703.811767	24.796032
154.037459	4693.378977	24.801050
154.158352	4714.701917	24.806067
154.544598	4725.612770	24.811085
155.013735	4718.079051	24.816103
154.833575	4726.318815	24.821120
155.091240	4720.222327	24.826138
155.359161	4731.839647	24.831155
155.601213	4738.315137	24.836173
156.210224	4741.771675	24.841191
156.234652	4733.143714	24.846208
156.513255	4728.578783	24.851226
156.606221	4713.399085	24.856243
156.286183	4731.593537	24.861261
156.617799	4716.906823	24.866279
156.579671	4720.543637	24.871296
156.530405	4725.045263	24.876314
156.902276	4717.103794	24.881331
156.797452	4736.815357	24.886349
156.997844	4733.754524	24.891367
157.131318	4759.420601	24.896384
157.366971	4754.661109	24.901402
157.325249	4764.974658	24.906419
157.262409	4769.105554	24.911437
157.416947	4792.414445	24.916455
157.897464	4788.591443	24.921472
157.903352	4804.357315	24.926490
158.525484	4810.119252	24.931507
158.685299	4814.350764	24.936525
159.047784	4807.093625	24.941543
158.831815	4811.695809	24.946560
159.190657	4803.798856	24.951578
159.842085	4809.519146	24.956595
159.487403	4811.223111	24.961613
159.967705	4810.198530	24.966631
160.182438	4821.132869	24.971648
160.059367	4830.308450	24.976666
160.512565	4827.247414	24.981683
160.352428	4824.844319	24.986701
160.229141	4822.030184	24.991719
160.371030	4828.793892	24.996736
160.358223	4822.391179	25.001754
160.527257	4829.900312	25.006771
160.470250	4857.214445	25.011789
160.717813	4859.049759	25.016807
160.807963	4870.309249	25.021824
160.575120	4889.390013	25.026842
161.102832	4890.436415	25.031859
161.507850	4907.420348	25.036877
162.347213	4890.746253	25.041895
162.509082	4902.958867	25.046912
162.764173	4892.162777	25.051930
162.952406	4896.453507	25.056947
162.891161	4890.772840	25.061965
162.872082	4886.483476	25.066983
162.995338	4893.154990	25.072000
163.124737	4888.057580	25.077018
163.042667	4881.908197	25.082035
163.060450	4895.665318	25.087053
163.599498	4890.635551	25.092071
163.508285	4894.643555	25.097088
163.284733	4897.176293	25.102106
163.900536	4901.479888	25.107123
163.887217	4914.327014	25.112141
164.013146	4909.560578	25.117159
164.582774	4905.006625	25.122176
165.009405	4922.515029	25.127194
165.320034	4910.098839	25.132211
165.125403	4931.622667	25.137229
165.443923	4910.945292	25.142247
165.210714	4919.483139	25.147264
165.173071	4923.613994	25.152282
165.746935	4922.500537	25.157299
165.633612	4924.289550	25.162317
165.778554	4921.510517	25.167335
165.963812	4935.240186	25.172352
166.127080	4949.034740	25.177370
166.309575	4952.172260	25.182387
166.192538	4955.892519	25.187405
166.662751	4964.032655	25.192423
166.554995	4969.701757	25.197440
166.708139	4990.215124	25.202458
167.087193	4980.054557	25.207475
167.066550	5003.998290	25.212493
167.189215	5012.805161	25.217511
167.505875	5018.354690	25.222528
167.668571	5033.018760	25.227546
168.134151	5037.102458	25.232563
168.185939	5047.372973	25.237581
168.103645	5052.643890	25.242599
168.238149	5053.367495	25.247616
168.218637	5062.048370	25.252634
168.565942	5069.207425	25.257651
168.615726	5080.051818	25.262669
168.806344	5093.057763	25.267687
168.875696	5106.277380	25.272704
169.050989	5115.407141	25.277722
169.089722	5130.679558	25.282739
169.278977	5145.750973	25.287757
169.858105	5151.471914	25.292775
169.842096	5170.856769	25.297792
169.833782	5177.351916	25.302810
170.572437	5180.318992	25.307827
170.254196	5205.595258	25.312845
170.293654	5198.830798	25.317863
170.558053	5219.526579	25.322880
171.039468	5226.731204	25.327898
171.008872	5230.034933	25.332915
171.122673	5237.495648	25.337933
171.358472	5251.028733	25.342951
171.554961	5271.157151	25.347968
171.455693	5262.728769	25.352986
171.811962	5283.416286	25.358003
171.870073	5296.427015	25.363021
171.788860	5293.897967	25.368039
172.275500	5314.131240	25.373056
172.625564	5323.285978	25.378074
172.866211	5323.317638	25.383091
172.874974	5345.817472	25.388109
173.066876	5353.192625	25.393127
173.393015	5349.329582	25.398144
172.954587	5365.778204	25.403162
173.022172	5379.216278	25.408179
173.349500	5396.955864	25.413197
173.706028	5422.185498	25.418215
173.993028	5424.662101	25.423232
174.542462	5438.452978	25.428250
174.719077	5438.200599	25.433267
174.953571	5443.865668	25.438285
174.778955	5452.288266	25.443303
175.111934	5454.080928	25.448320
175.199343	5481.827152	25.453338
175.571044	5484.077049	25.458355
175.497946	5482.797629	25.463373
175.645157	5488.914072	25.468391
176.019228	5506.051544	25.473408
176.134934	5518.023410	25.478426
176.507238	5511.972837	25.483443
176.499485	5522.544278	25.488461
176.818404	5529.633342	25.493479
177.352793	5528.052506	25.498496
176.864755	5534.655763	25.503514
177.139228	5542.573304	25.508531
177.252858	5558.923894	25.513549
177.078096	5561.404119	25.518567
177.630331	5570.969730	25.523584
177.466600	5585.065631	25.528602
177.915522	5588.575439	25.533619
177.602436	5609.709229	25.538637
177.652001	5627.050424	25.543655
178.334491	5642.508692	25.548672
178.476721	5663.568392	25.553690
179.019592	5654.073611	25.558707
179.357399	5671.971573	25.563725
179.396240	5683.389350	25.568743
179.061183	5691.001321	25.573760
179.475732	5703.484302	25.578778
179.884155	5705.545060	25.583795
180.114621	5717.328061	25.588813
180.276268	5721.288105	25.593831
180.158082	5737.815898	25.598848
180.369018	5754.555594	25.603866
180.566063	5749.227593	25.608883
180.400547	5761.096577	25.613901
180.513272	5780.054940	25.618919
181.032407	5785.595296	25.623936
181.022098	5806.198796	25.628954
181.560022	5810.374248	25.633971
181.602596	5818.601136	25.638989
182.092064	5833.375194	25.644007
182.390096	5841.337133	25.649024
182.219250	5852.654718	25.654042
182.721563	5843.043546	25.659059
182.628552	5844.829430	25.664077
182.806915	5862.886009	25.669095
183.119736	5870.615866	25.674112
182.921968	5872.218611	25.679130
183.406815	5891.538720	25.684148
183.115094	5911.077863	25.689165
183.512417	5912.727359	25.694183
183.972856	5917.294426	25.699200
183.876983	5935.734708	25.704218
184.140581	5931.820119	25.709236
184.545330	5950.555116	25.714253
184.683729	5968.806239	25.719271
184.674737	5962.777722	25.724288
184.833684	5986.852555	25.729306
185.000336	5998.021242	25.734324
185.207974	5998.826864	25.739341
185.222332	6019.012088	25.744359
185.715012	6028.940763	25.749376
185.641055	6046.200645	25.754394
185.862868	6052.632735	25.759412
186.354655	6061.452981	25.764429
186.480793	6068.720958	25.769447
186.701390	6078.228835	25.774464
186.744749	6097.588914	25.779482
186.938923	6100.321193	25.784500
187.040668	6108.825989	25.789517
187.044964	6127.009778	25.794535
187.680139	6129.234295	25.799552
188.112884	6148.683427	25.804570
188.023927	6160.335956	25.809588
188.752146	6143.547582	25.814605
189.213853	6138.829505	25.819623
189.735700	6130.458178	25.824640
189.749848	6126.325237	25.829658
189.486280	6131.522366	25.834676
189.861292	6123.888865	25.839693
189.812134	6133.137654	25.844711
190.079522	6127.194043	25.849728
189.671999	6132.458182	25.854746
189.823141	6130.179915	25.859764
190.096903	6130.592619	25.864781
190.218291	6154.918407	25.869799
190.300113	6159.120255	25.874816
190.356465	6168.650442	25.879834
190.508120	6177.914451	25.884852
190.972801	6184.716229	25.889869
190.380972	6205.601039	25.894887
191.341053	6216.952611	25.899904
191.081937	6222.791879	25.904922
191.317730	6243.780051	25.909940
191.519226	6247.748834	25.914957
191.696577	6269.821923	25.919975
191.956430	6274.069380	25.924992
192.301144	6285.250023	25.930010
192.266281	6298.707625	25.935028
192.682321	6317.620680	25.940045
192.843799	6323.093946	25.945063
193.279922	6327.596568	25.950080
193.249883	6342.367411	25.955098
193.347434	6353.538728	25.960116
193.716539	6365.958704	25.965133
193.835589	6376.585284	25.970151
193.984913	6386.924581	25.975168
194.265206	6393.471026	25.980186
194.556368	6406.956217	25.985204
194.991478	6424.089745	25.990221
194.502215	6425.059212	25.995239
194.880996	6438.838894	26.000256
194.866324	6446.342733	26.005274
195.358838	6467.664818	26.010292
195.758175	6478.638622	26.015309
195.644213	6475.196376	26.020327
196.134046	6501.818936	26.025344
196.137432	6515.224214	26.030362
196.149618	6517.758981	26.035380
196.816466	6512.715387	26.040397
196.705598	6534.151073	26.045415
197.216723	6533.445645	26.050432
197.571015	6562.167126	26.055450
197.286515	6557.169752	26.060468
197.399891	6561.614532	26.065485
198.071787	6568.642318	26.070503
198.189409	6575.279297	26.075520
198.081344	6590.002240	26.080538
198.530481	6605.612027	26.085556
199.136429	6606.620918	26.090573
199.393540	6610.116707	26.095591
199.543763	6610.479881	26.100608
199.680523	6616.457617	26.105626
199.575382	6616.892188	26.110644
199.780903	6627.100735	26.115661
200.021880	6635.333427	26.120679
200.337508	6633.944725	26.125696
200.148216	6639.913865	26.130714
200.090107	6663.950439	26.135732
200.701920	6662.243061	26.140749
200.823588	6671.376826	26.145767
201.050935	6686.711261	26.150784
201.181398	6684.983839	26.155802
201.309955	6698.466107	26.160820
201.558114	6692.124056	26.165837
201.916423	6718.473700	26.170855
202.200157	6722.295740	26.175872
202.231021	6734.725101	26.180890
202.226875	6726.279933	26.185908
202.359443	6743.541533	26.190925
202.381876	6767.511930	26.195943
202.578249	6765.716553	26.200960
202.903951	6795.890815	26.205978
203.043093	6803.193275	26.210996
203.713196	6809.285918	26.216013
203.801222	6826.276176	26.221031
203.984834	6824.106719	26.226048
203.768359	6850.309032	26.231066
203.984602	6857.836064	26.236084
204.373270	6868.997553	26.241101
204.277663	6880.854709	26.246119
204.833747	6898.316497	26.251136
205.224030	6905.804005	26.256154
205.099580	6915.776586	26.261172
205.610485	6920.381562	26.266189
205.764893	6932.895255	26.271207
206.223121	6932.306829	26.276224
206.467669	6932.682514	26.281242
206.581485	6959.882404	26.286260
207.341100	6947.424812	26.291277
207.187661	6966.818577	26.296295
207.212597	6958.662921	26.301312
207.908212	6954.470289	26.306330
207.901638	6981.736622	26.311348
208.072792	6978.737435	26.316365
208.035553	6988.397947	26.321383
208.718193	6974.301412	26.326400
208.709221	6979.328416	26.331418
208.432897	6992.706325	26.336436
208.917633	6998.788471	26.341453
208.918329	7002.717867	26.346471
208.939128	7020.544464	26.351488
209.091016	7029.488723	26.356506
209.511194	7045.911684	26.361524
209.719817	7042.820745	26.366541
209.816412	7065.316264	26.371559
210.137586	7088.825671	26.376576
210.506009	7087.567786	26.381594
210.510983	7109.658587	26.386612
210.833313	7111.707311	26.391629
210.740456	7120.621399	26.396647
210.897938	7142.039571	26.401664
211.146444	7147.520514	26.406682
211.156768	7167.665450	26.411700
211.495301	7172.272807	26.416717
211.464808	7197.585263	26.421735
211.790095	7212.406549	26.426752
212.214678	7228.327782	26.431770
212.382164	7250.609270	26.436788
212.506803	7251.563536	26.441805
212.190919	7279.282200	26.446823
212.635216	7285.049873	26.451840
213.018126	7306.208875	26.456858
213.201033	7318.679007	26.461876
213.687384	7337.126564	26.466893
213.913071	7348.851038	26.471911
214.427441	7356.883175	26.476928
214.686607	7359.776866	26.481946
214.455173	7380.280882	26.486964
214.878146	7372.782313	26.491981
214.960169	7402.577256	26.496999
215.014268	7414.306316	26.502016
215.211067	7419.286501	26.507034
215.287850	7434.843214	26.512052
215.751019	7451.461995	26.517069
215.814025	7476.804870	26.522087
216.304617	7482.680124	26.527104
216.473467	7489.349476	26.532122
216.448990	7510.475354	26.537140
216.954877	7516.590540	26.542157
217.401673	7533.383561	26.547175
217.290722	7541.367553	26.552192
217.565690	7558.523202	26.557210
218.006810	7569.133916	26.562228
218.214785	7581.830826	26.567245
218.116840	7599.680192	26.572263
218.650682	7602.877942	26.577280
219.271876	7604.338509	26.582298
219.453933	7602.092862	26.587316
219.876231	7598.104545	26.592333
220.417907	7599.300807	26.597351
220.060580	7608.461147	26.602368
220.532222	7591.321774	26.607386
220.519919	7607.555419	26.612404
221.009953	7619.231670	26.617421
221.067652	7631.671665	26.622439
221.163374	7634.556843	26.627456
221.544389	7624.125063	26.632474
221.249484	7633.580776	26.637492
221.840915	7649.349177	26.642509
222.156299	7657.035499	26.647527
222.432512	7655.069914	26.652544
222.437741	7652.132455	26.657562
222.324795	7661.900683	26.662580
222.789190	7664.379295	26.667597
223.326173	7675.168376	26.672615
223.359018	7678.445223	26.677632
223.698651	7675.271894	26.682650
223.292981	7689.894643	26.687668
223.685685	7696.262437	26.692685
223.804417	7707.415658	26.697703
223.705903	7724.889135	26.702720
224.258798	7733.755729	26.707738
224.528127	7755.780165	26.712756
224.615216	7768.053490	26.717773
224.666583	7788.858426	26.722791
224.658661	7786.131561	26.727808
225.001415	7799.182517	26.732826
225.139922	7818.573732	26.737844
225.377755	7835.337456	26.742861
225.543402	7838.252839	26.747879
225.944662	7877.259913	26.752896
226.125748	7872.802432	26.757914
225.955390	7901.782467	26.762932
226.170916	7915.379450	26.767949
226.643632	7934.844623	26.772967
226.694378	7954.127248	26.777984
227.214962	7958.983212	26.783002
227.463369	7976.983589	26.788020
228.014039	7996.639435	26.793037
228.259495	8010.488262	26.798055
228.137548	8030.189996	26.803072
228.536070	8048.713818	26.808090
228.667097	8060.960706	26.813108
228.961850	8076.517572	26.818125
229.197561	8079.256977	26.823143
229.266083	8098.718337	26.828160
230.519355	8095.106157	26.833178
230.774583	8100.317262	26.838196
231.421365	8101.295369	26.843213
231.908386	8105.276975	26.848231
231.719585	8096.878960	26.853248
232.123741	8103.186088	26.858266
232.275534	8099.994221	26.863284
232.128068	8093.044994	26.868301
232.481026	8098.060713	26.873319
231.976671	8104.432796	26.878336
232.442480	8087.567630	26.883354
232.442299	8106.382495	26.888372
232.666184	8120.886813	26.893389
233.169172	8127.793555	26.898407
233.068262	8134.100944	26.903424
233.524785	8148.562302	26.908442
233.289496	8171.165117	26.913460
233.754292	8182.951283	26.918477
233.793131	8187.008684	26.923495
233.905882	8208.470143	26.928512
234.434219	8225.036517	26.933530
234.240784	8247.067379	26.938548
234.645018	8261.894047	26.943565
234.916749	8277.849822	26.948583
235.094226	8298.596413	26.953600
235.570449	8307.867851	26.958618
235.562106	8331.655232	26.963636
235.854509	8349.566026	26.968653
236.265336	8360.573628	26.973671
236.400280	8377.987437	26.978688
236.869675	8392.682269	26.983706
236.891307	8401.863733	26.988724
237.107301	8409.850366	26.993741
237.400695	8434.891769	26.998759
237.268549	8450.317986	27.003776
237.433801	8455.087538	27.008794
237.719124	8480.033512	27.013812
237.633456	8491.585426	27.018829
238.101788	8510.362706	27.023847
238.200409	8535.986567	27.028864
238.644094	8544.049901	27.033882
239.862901	8550.891918	27.038900
240.175679	8550.270757	27.043917
240.424373	8554.317627	27.048935
240.249423	8556.956935	27.053952
240.918135	8564.213223	27.058970
241.197742	8576.882644	27.063988
241.216266	8582.146603	27.069005
241.539058	8570.054773	27.074023
241.391963	8585.942683	27.079040
241.871252	8593.068647	27.084058
242.045789	8602.263632	27.089076
242.015118	8610.587940	27.094093
242.142185	8617.764159	27.099111
242.514889	8628.641505	27.104128
242.730277	8631.398811	27.109146
242.775968	8668.212044	27.114164
243.218746	8683.834085	27.119181
243.506072	8690.978105	27.124199
243.514099	8707.217570	27.129216
243.828824	8715.982647	27.134234
244.158498	8735.373302	27.139252
243.993891	8745.748149	27.144269
244.305140	8762.247031	27.149287
244.004627	8780.123797	27.154304
244.890919	8802.817909	27.159322
245.132050	8826.966074	27.164340
245.276902	8841.707574	27.169357
245.681220	8855.227316	27.174375
245.259245	8879.664625	27.179392
245.650560	8901.795249	27.184410
246.152724	8921.117335	27.189428
246.411250	8936.166603	27.194445
246.768454	8959.456808	27.199463
247.076972	8967.778003	27.204480
247.425239	8989.821580	27.209498
247.728962	9007.876157	27.214516
248.027498	9032.558498	27.219533
248.422523	9029.361896	27.224551
248.251607	9046.823271	27.229568
248.784808	9063.503911	27.234586
249.277561	9069.990527	27.239604
249.318067	9093.713094	27.244621
249.558002	9096.270624	27.249639
249.612405	9118.655947	27.254656
249.881342	9122.872483	27.259674
250.342489	9141.512412	27.264692
250.333830	9155.920626	27.269709
250.675656	9156.924996	27.274727
250.995511	9188.754889	27.279744
251.015611	9194.098687	27.284762
251.298658	9201.590290	27.289780
251.343923	9225.498423	27.294797
251.779224	9235.240092	27.299815
251.782290	9262.695552	27.304832
252.116945	9269.641861	27.309850
252.434461	9292.696918	27.314868
252.655489	9305.422332	27.319885
253.329282	9326.030243	27.324903
253.516850	9340.154738	27.329920
253.723989	9352.974088	27.334938
253.891254	9354.725980	27.339956
253.783954	9380.550943	27.344973
254.592067	9388.690039	27.349991
254.736223	9404.503663	27.355008
255.153389	9414.624905	27.360026
255.437825	9422.490603	27.365044
255.293288	9444.341896	27.370061
256.058822	9457.847497	27.375079
255.987829	9474.263290	27.380096
255.847775	9483.158759	27.385114
256.464788	9496.150171	27.390132
256.055962	9517.870564	27.395149
256.734024	9532.037069	27.400167
256.970014	9552.916544	27.405184
257.188113	9570.092621	27.410202
257.522364	9598.624826	27.415220
257.936821	9609.166486	27.420237
258.400594	9616.476815	27.425255
258.736874	9653.032475	27.430272
258.958057	9659.376122	27.435290
259.255169	9660.374671	27.440308
259.452158	9672.564358	27.445325
259.508720	9686.756100	27.450343
259.719738	9708.503882	27.455360
260.199246	9708.006418	27.460378
260.543257	9737.785886	27.465396
260.501014	9755.009180	27.470413
261.094398	9764.395069	27.475431
261.293236	9787.345852	27.480448
261.217662	9792.210490	27.485466
261.654401	9807.219242	27.490484
262.078564	9831.424056	27.495501
262.130144	9848.237825	27.500519
262.343132	9844.820988	27.505536
262.585762	9863.052390	27.510554
262.669616	9886.432070	27.515572
262.971937	9909.131627	27.520589
263.268211	9911.411951	27.525607
263.182084	9949.520725	27.530624
263.585116	9963.842447	27.535642
264.104243	9982.222342	27.540660
264.325200	9997.551754	27.545677
264.654855	10004.727826	27.550695
264.960901	10016.860272	27.555712
265.222723	10040.532528	27.560730
265.605521	10048.543426	27.565748
265.706506	10066.924753	27.570765
265.703079	10075.871590	27.575783
266.008925	10090.776356	27.580800
266.542508	10113.153281	27.585818
266.882092	10115.154036	27.590836
266.859215	10141.244659	27.595853
266.916334	10139.807139	27.600871
267.435753	10166.393752	27.605888
267.698263	10193.962629	27.610906
268.195997	10205.337868	27.615924
268.187562	10229.269140	27.620941
268.710103	10231.411137	27.625959
269.081567	10246.750065	27.630976
269.558703	10260.990215	27.635994
270.065169	10258.529953	27.641012
270.329223	10279.453185	27.646029
270.738658	10283.491827	27.651047
271.019692	10288.552022	27.656064
271.330198	10284.088552	27.661082
271.873349	10290.152126	27.666100
271.660353	10301.066595	27.671117
272.030579	10304.117490	27.676135
272.278615	10314.187206	27.681152
272.010035	10315.018614	27.686170
272.240967	10321.418834	27.691188
272.451886	10342.116879	27.696205
272.881342	10358.357850	27.701223
273.052528	10375.776463	27.706240
273.251601	10391.620936	27.711258
273.683416	10401.825512	27.716276
273.904195	10426.695683	27.721293
274.413278	10423.375942	27.726311
274.788031	10428.824990	27.731328
274.826328	10463.923358	27.736346
275.658290	10472.490151	27.741364
275.728871	10465.454304	27.746381
275.777779	10485.093452	27.751399
275.895673	10499.439492	27.756416
276.288457	10500.996989	27.761434
277.256830	10517.386375	27.766452
276.597962	10535.106293	27.771469
277.162793	10527.462361	27.776487
277.377155	10542.341232	27.781504
277.645155	10551.761774	27.786522
277.805418	10557.388690	27.791540
277.966078	10580.903594	27.796557
278.447532	10589.885209	27.801575
278.741055	10609.331665	27.806592
278.772333	10626.098774	27.811610
279.348430	10632.832907	27.816628
279.408174	10653.315036	27.821645
279.343339	10662.848513	27.826663
279.684600	10678.385324	27.831680
279.750847	10695.792700	27.836698
280.221791	10711.462740	27.841716
280.509937	10726.118319	27.846733
280.870195	10746.159548	27.851751
280.869304	10757.428549	27.856768
281.272545	10779.529743	27.861786
281.688970	10793.369634	27.866804
281.719533	10819.850367	27.871821
282.123065	10832.887204	27.876839
282.756622	10845.041314	27.881856
282.554381	10861.206822	27.886874
283.347521	10875.044593	27.891892
283.499118	10902.441979	27.896909
283.851661	10908.912397	27.901927
284.320367	10921.832672	27.906944
284.826042	10925.587767	27.911962
285.484564	10933.221091	27.916980
285.647536	10934.141549	27.921997
285.882618	10939.220702	27.927015
286.615767	10951.524307	27.932032
286.283876	10975.502806	27.937050
286.519404	10971.279333	27.942068
286.574042	10964.368182	27.947085
287.000550	10978.982671	27.952103
287.010619	10986.589514	27.957120
286.859113	11018.950964	27.962138
287.200934	11023.190660	27.967156
287.562048	11043.195551	27.972173
287.759447	11072.090009	27.977191
288.433432	11084.672327	27.982208
288.520086	11098.908218	27.987226
288.988966	11118.986938	27.992244
289.060034	11138.345178	27.997261
289.033928	11161.312853	28.002279
289.539235	11173.049278	28.007296
289.688349	11205.453723	28.012314
290.002362	11221.632764	28.017332
290.174174	11248.001614	28.022349
290.370915	11274.201646	28.027367
290.977281	11286.314209	28.032384
291.074374	11309.392929	28.037402
291.596927	11334.461867	28.042420
291.767341	11366.651933	28.047437
292.405430	11372.627032	28.052455
293.012428	11384.414512	28.057472
293.044665	11407.749877	28.062490
294.612243	11386.234267	28.067508
295.308836	11387.423494	28.072525
295.302335	11391.781778	28.077543
295.662744	11384.534813	28.082560
296.147617	11387.201278	28.087578
296.187887	11371.242655	28.092596
296.302447	11356.766464	28.097613
296.426239	11348.645012	28.102631
296.566246	11342.462882	28.107648
296.245279	11348.005248	28.112666
296.545682	11349.691295	28.117684
296.514743	11368.269570	28.122701
296.719443	11382.425129	28.127719
297.186422	11396.181961	28.132736
297.214546	11405.408691	28.137754
297.490640	11421.738812	28.142772
297.651480	11451.185265	28.147789
297.728308	11464.906548	28.152807
298.008339	11475.890071	28.157824
298.243503	11512.317992	28.162842
298.834654	11527.813688	28.167860
298.868953	11540.013305	28.172877
299.074845	11579.493242	28.177895
299.458730	11595.255215	28.182912
299.600563	11622.682223	28.187930
299.886700	11646.613257	28.192948
300.300968	11675.523496	28.197965
300.193490	11705.885500	28.202983
300.551651	11718.092675	28.208000
300.776640	11761.932101	28.213018
301.317677	11785.563185	28.218036
301.749828	11810.812809	28.223053
302.007375	11843.547069	28.228071
302.790947	11864.662822	28.233088
302.871797	11889.556325	28.238106
303.312247	11912.720753	28.243124
304.006729	11936.905743	28.248141
304.040660	11950.283057	28.253159
304.544272	11964.676255	28.258176
304.594774	11988.084178	28.263194
304.794388	12010.582877	28.268212
305.647991	12030.421641	28.273229
305.778273	12047.001969	28.278247
306.444117	12058.498030	28.283264
306.581761	12079.955329	28.288282
306.727056	12085.504917	28.293300
306.953725	12104.623922	28.298317
307.153899	12121.963972	28.303335
307.809428	12136.153660	28.308352
307.982196	12153.714373	28.313370
308.128274	12173.492334	28.318388
308.593937	12187.456715	28.323405
308.559086	12211.959099	28.328423
309.104664	12230.611052	28.333440
309.105143	12248.436650	28.338458
309.791499	12265.870773	28.343476
309.947273	12276.509064	28.348493
310.114246	12307.171710	28.353511
310.467390	12322.706156	28.358528
310.955745	12338.675994	28.363546
311.181193	12354.107443	28.368564
311.576371	12362.678040	28.373581
311.817599	12384.411480	28.378599
312.108536	12390.630836	28.383616
312.276509	12417.932125	28.388634
312.738665	12432.300694	28.393652
312.910911	12446.965395	28.398669
313.135711	12471.397298	28.403687
313.734268	12485.640081	28.408704
313.703261	12506.166332	28.413722
314.198143	12514.732341	28.418740
314.588584	12536.042748	28.423757
314.594430	12554.368465	28.428775
314.863009	12565.497469	28.433792
315.184701	12595.412661	28.438810
315.506312	12616.821523	28.443828
315.724928	12643.233551	28.448845
316.146540	12669.729179	28.453863
316.810141	12694.567923	28.458880
316.973163	12709.036381	28.463898
316.984004	12735.825468	28.468916
317.491162	12764.652333	28.473933
317.503735	12789.432640	28.478951
317.922633	12802.170108	28.483968
318.633271	12824.809856	28.488986
318.984620	12840.017862	28.494004
319.619284	12858.782729	28.499021
319.672358	12875.223755	28.504039
320.565290	12896.043100	28.509056
320.412217	12912.848806	28.514074
320.310881	12933.267979	28.519092
320.908160	12952.580679	28.524109
321.295243	12975.927723	28.529127
321.610734	12984.436495	28.534144
321.838352	13005.857539	28.539162
322.295331	13029.356467	28.544180
323.011774	13043.236311	28.549197
322.977605	13056.837000	28.554215
323.433777	13062.450753	28.559232
323.509835	13086.613934	28.564250
323.774746	13101.477917	28.569268
324.588369	13111.790956	28.574285
324.414684	13138.856270	28.579303
324.794367	13161.101763	28.584320
325.081198	13177.286241	28.589338
325.040654	13201.777544	28.594356
325.617753	13219.635769	28.599373
325.647496	13259.715687	28.604391
326.395212	13268.786555	28.609408
326.442640	13296.253764	28.614426
326.626301	13323.863141	28.619444
326.847829	13347.125557	28.624461
327.096159	13386.506595	28.629479
327.642892	13411.544221	28.634496
327.976261	13438.000050	28.639514
328.321786	13466.386615	28.644532
328.508663	13484.195758	28.649549
329.157156	13494.412477	28.654567
329.589258	13513.714823	28.659584
330.007129	13532.999095	28.664602
330.485411	13557.561586	28.669620
330.791135	13570.420958	28.674637
331.203058	13585.775920	28.679655
331.161052	13600.149883	28.684672
331.659603	13624.839041	28.689690
331.670291	13632.132526	28.694708
332.052167	13643.070787	28.699725
332.349386	13678.071550	28.704743
332.230855	13692.467536	28.709760
332.425836	13719.588651	28.714778
332.692446	13747.322448	28.719796
333.317723	13771.163713	28.724813
333.825699	13813.649818	28.729831
333.648414	13833.820946	28.734848
334.307483	13872.450060	28.739866
334.940361	13897.736797	28.744884
335.389018	13924.666213	28.749901
335.154954	13956.250374	28.754919
335.917659	13982.775699	28.759936
336.279877	14012.418479	28.764954
336.828420	14034.157449	28.769972
337.203028	14040.715147	28.774989
337.731897	14069.452264	28.780007
338.091153	14083.859757	28.785024
338.693594	14099.792801	28.790042
338.704229	14124.434865	28.795060
339.326221	14131.714908	28.800077
339.759340	14144.595888	28.805095
340.391263	14158.420559	28.810112
340.623053	14165.556552	28.815130
340.621819	14197.698479	28.820148
341.053468	14196.162024	28.825165
341.141559	14220.612316	28.830183
341.502272	14233.443211	28.835200
341.812649	14251.625406	28.840218
342.247277	14270.865530	28.845236
342.612088	14287.974276	28.850253
342.841171	14310.317772	28.855271
343.100512	14328.131504	28.860288
343.399512	14350.609258	28.865306
343.378978	14362.660360	28.870324
344.104585	14383.800182	28.875341
344.424173	14402.220406	28.880359
344.538498	14427.009094	28.885376
345.143619	14451.876955	28.890394
345.399956	14466.850404	28.895412
345.919132	14485.042507	28.900429
345.925324	14510.868128	28.905447
346.463075	14540.385555	28.910464
346.952591	14555.421713	28.915482
346.816011	14574.946811	28.920500
347.249116	14595.903176	28.925517
347.716599	14612.258772	28.930535
347.972511	14638.368171	28.935552
348.390801	14654.026185	28.940570
348.559727	14680.578762	28.945588
349.162309	14698.223879	28.950605
349.464294	14713.115900	28.955623
349.702880	14737.112900	28.960640
350.376572	14751.245960	28.965658
350.502636	14770.591485	28.970676
350.793273	14792.814578	28.975693
351.229369	14800.009238	28.980711
351.606151	14832.321342	28.985728
351.970573	14837.727195	28.990746
352.004061	14866.599468	28.995764
352.522182	14884.579263	29.000781
352.610482	14912.426248	29.005799
353.070702	14946.600933	29.010816
353.612699	14959.864687	29.015834
353.521968	14991.317448	29.020852
354.309760	15020.082795	29.025869
354.608512	15048.525510	29.030887
354.790120	15077.462650	29.035904
355.404720	15098.527470	29.040922
355.710286	15120.966929	29.045940
356.529983	15143.350272	29.050957
356.675862	15156.734497	29.055975
356.939507	15182.256976	29.060992
357.583421	15197.775771	29.066010
357.611886	15221.310835	29.071028
358.199623	15232.525356	29.076045
358.781228	15252.417001	29.081063
359.247197	15275.448248	29.086080
359.778664	15285.585927	29.091098
359.393038	15303.754123	29.096116
360.139954	15314.330641	29.101133
360.127588	15339.907502	29.106151
360.446479	15356.977230	29.111168
361.370999	15370.453176	29.116186
361.529160	15392.992003	29.121204
361.766010	15412.871090	29.126221
362.310884	15431.082465	29.131239
362.603104	15450.949235	29.136256
362.825784	15471.331958	29.141274
362.939740	15502.875470	29.146292
363.512707	15518.000642	29.151309
363.878972	15528.683040	29.156327
363.998053	15559.863503	29.161344
364.357548	15583.888024	29.166362
364.658648	15615.595225	29.171380
364.745769	15636.608738	29.176397
365.277066	15667.392871	29.181415
365.602486	15683.841141	29.186432
366.019465	15716.376228	29.191450
366.164893	15750.814255	29.196468
366.683797	15768.929002	29.201485
367.072763	15782.235768	29.206503
366.872356	15812.706728	29.211520
367.519431	15842.014678	29.216538
367.634634	15869.209088	29.221556
367.738153	15893.134545	29.226573
368.469375	15920.779634	29.231591
368.664989	15956.898110	29.236608
369.602708	15994.874172	29.241626
370.106502	16026.653056	29.246644
370.258426	16037.070982	29.251661
370.705582	16060.297327	29.256679
370.858149	16101.198652	29.261696
371.617705	16116.163003	29.266714
372.118151	16138.838711	29.271732
372.598081	16166.696906	29.276749
372.754835	16185.839045	29.281767
373.244086	16212.531193	29.286784
373.434051	16225.764947	29.291802
373.738487	16259.236345	29.296820
374.065271	16287.837990	29.301837
374.890895	16310.669988	29.306855
374.827256	16338.065556	29.311872
375.214471	16357.763845	29.316890
375.573912	16384.386040	29.321908
375.605958	16417.308719	29.326925
375.925535	16450.670649	29.331943
376.398352	16481.925138	29.336960
376.832799	16513.338351	29.341978
376.980937	16557.879285	29.346996
377.733489	16577.959566	29.352013
378.270791	16616.999317	29.357031
378.122714	16648.962682	29.362048
378.976295	16666.486811	29.367066
379.783378	16687.850579	29.372084
380.380085	16708.450318	29.377101
380.891904	16730.601105	29.382119
381.602740	16742.366767	29.387136
382.410096	16756.557054	29.392154
382.308864	16765.035233	29.397172
382.631495	16777.758196	29.402189
383.275961	16792.634075	29.407207
383.327625	16802.622854	29.412224
383.508266	16812.734581	29.417242
383.702280	16839.595326	29.422260
384.163316	16859.136439	29.427277
384.446072	16870.596616	29.432295
384.697852	16895.061778	29.437312
385.272630	16910.676394	29.442330
385.253249	16940.097160	29.447348
385.660930	16960.911402	29.452365
385.994271	16984.561389	29.457383
385.948071	17018.222580	29.462400
386.447514	17038.185732	29.467418
387.073808	17069.521084	29.472436
387.073047	17107.743917	29.477453
387.642176	17126.997291	29.482471
387.651522	17161.626278	29.487488
388.258660	17183.748749	29.492506
388.510772	17209.575326	29.497524
388.782087	17248.871647	29.502541
389.248121	17265.802332	29.507559
389.401834	17301.921964	29.512576
389.800987	17336.294745	29.517594
389.965195	17373.169935	29.522612
391.025816	17407.150866	29.527629
391.420200	17440.121521	29.532647
391.448877	17480.625176	29.537664
392.271472	17511.918335	29.542682
392.679915	17545.800344	29.547700
393.017153	17574.679273	29.552717
393.739383	17593.341518	29.557735
394.044703	17627.400766	29.562752
394.821193	17654.545303	29.567770
394.867197	17675.585065	29.572788
395.030012	17701.008975	29.577805
395.539767	17732.546915	29.582823
395.660947	17761.831484	29.587840
396.386291	17791.222203	29.592858
396.860193	17821.567217	29.597876
397.137972	17855.417180	29.602893
397.577828	17870.106625	29.607911
398.108642	17892.579282	29.612928
398.781943	17910.770570	29.617946
399.176011	17933.152083	29.622964
399.594308	17956.458123	29.627981
399.866978	17982.634684	29.632999
400.319090	18008.998053	29.638016
400.774323	18021.381615	29.643034
401.200828	18048.917262	29.648052
401.352755	18081.597198	29.653069
401.592876	18098.486838	29.658087
401.989203	18129.797198	29.663104
402.630190	18149.475840	29.668122
403.214310	18186.222663	29.673140
403.488170	18203.205862	29.678157
403.867804	18226.501933	29.683175
404.024234	18259.769338	29.688192
404.796723	18278.259439	29.693210
405.421127	18299.640575	29.698228
405.529491	18331.702366	29.703245
405.784925	18344.529061	29.708263
406.003962	18372.400711	29.713280
406.392801	18404.588441	29.718298
406.736289	18437.626807	29.723316
406.914642	18477.169401	29.728333
407.307743	18509.691330	29.733351
407.554153	18553.471504	29.738368
407.898499	18573.492059	29.743386
408.906215	18587.290483	29.748404
409.449149	18616.766559	29.753421
410.083427	18630.007561	29.758439
410.755722	18643.648839	29.763456
411.243770	18660.664162	29.768474
411.907995	18679.753916	29.773492
411.752148	18688.272553	29.778509
412.388970	18705.080351	29.783527
412.691558	18714.351991	29.788544
413.235273	18728.477638	29.793562
413.712193	18741.389063	29.798580
413.996557	18769.638047	29.803597
414.730737	18762.967117	29.808615
414.809128	18789.863436	29.813632
414.784546	18815.441474	29.818650
415.234809	18839.752082	29.823668
415.285156	18862.246002	29.828685
415.565259	18886.468433	29.833703
416.091333	18929.809014	29.838720
416.313933	18951.074740	29.843738
416.769856	18983.478193	29.848756
416.771555	19027.852275	29.853773
417.574555	19052.060158	29.858791
417.752676	19100.617310	29.863808
418.199709	19136.008575	29.868826
418.273153	19166.082982	29.873844
418.800916	19214.286720	29.878861
419.557631	19244.472905	29.883879
419.806540	19282.036426	29.888896
420.355744	19321.827218	29.893914
420.928729	19357.675736	29.898932
421.240638	19399.133438	29.903949
421.932016	19427.141578	29.908967
422.110078	19467.160396	29.913984
422.759181	19506.163217	29.919002
423.125395	19537.539478	29.924020
423.063204	19575.674983	29.929037
423.581772	19606.372307	29.934055
424.170493	19658.508320	29.939072
424.914999	19683.176559	29.944090
425.360644	19726.262445	29.949108
425.439281	19755.881982	29.954125
426.453649	19783.874345	29.959143
427.424914	19818.565047	29.964160
427.411933	19837.055368	29.969178
428.021773	19862.157212	29.974196
428.298332	19894.261953	29.979213
428.557866	19918.223082	29.984231
428.834628	19949.404549	29.989248
429.282863	19980.565846	29.994266
430.067744	20011.982273	29.999284
430.333118	20036.357278	30.004301
430.660145	20063.583939	30.009319
431.191370	20097.365701	30.014336
431.412304	20119.964582	30.019354
431.915400	20138.365945	30.024372
432.181285	20168.759699	30.029389
432.814512	20203.509840	30.034407
433.008505	20221.267528	30.039424
433.578104	20253.078639	30.044442
434.096852	20266.290227	30.049460
434.442205	20301.555818	30.054477
435.057623	20324.429205	30.059495
435.623700	20336.288998	30.064512
436.191015	20359.235465	30.069530
436.787736	20375.274561	30.074548
437.157073	20405.686156	30.079565
437.369134	20420.762002	30.084583
437.643899	20444.508087	30.089600
437.968105	20468.015583	30.094618
438.467838	20503.276720	30.099636
438.504392	20536.812201	30.104653
438.827691	20570.337509	30.109671
439.160813	20595.151094	30.114688
439.819618	20628.842796	30.119706
440.790476	20663.686651	30.124724
440.807987	20710.031834	30.129741
441.135925	20735.919109	30.134759
441.306812	20778.215676	30.139776
441.613006	20807.428428	30.144794
442.343848	20838.757470	30.149812
442.518857	20884.068426	30.154829
443.041421	20926.111683	30.159847
443.489662	20969.685313	30.164864
443.793072	21016.701741	30.169882
444.446432	21053.126495	30.174900
444.737684	21095.734727	30.179917
445.057220	21146.711229	30.184935
445.671303	21190.817436	30.189952
446.090595	21227.660283	30.194970
446.640638	21267.590950	30.199988
447.011638	21314.041467	30.205005
447.576810	21351.421330	30.210023
448.273323	21396.553013	30.215040
448.490736	21432.556647	30.220058
449.294487	21460.248485	30.225076
449.905875	21511.554560	30.230093
450.371141	21528.135589	30.235111
451.089225	21556.654826	30.240128
451.290976	21588.005073	30.245146
451.637413	21619.852143	30.250164
451.870637	21655.360733	30.255181
452.389493	21690.122147	30.260199
452.723290	21726.312685	30.265216
453.278682	21763.120923	30.270234
453.833559	21794.540550	30.275252
454.388924	21838.185362	30.280269
454.938764	21870.454981	30.285287
455.227746	21904.197309	30.290304
455.704089	21947.844775	30.295322
456.244286	21968.811562	30.300340
456.628231	22006.803110	30.305357
456.800665	22029.508547	30.310375
457.258825	22056.894979	30.315392
457.704209	22082.039572	30.320410
458.332715	22116.113406	30.325428
458.500439	22159.537321	30.330445
459.213751	22187.333061	30.335463
459.889885	22209.741915	30.340480
459.627141	22250.526809	30.345498
460.589755	22283.276548	30.350516
460.862934	22321.848865	30.355533
461.285438	22365.014580	30.360551
461.889414	22391.841198	30.365568
462.175062	22429.425674	30.370586
462.661597	22461.993286	30.375604
463.073177	22507.522462	30.380621
463.642733	22550.714877	30.385639
463.977494	22578.700788	30.390656
463.845762	22624.041968	30.395674
464.860653	22654.789049	30.400692
465.376270	22700.712569	30.405709
465.941501	22738.128788	30.410727
466.695201	22767.751190	30.415744
467.304786	22804.637500	30.420762
467.631015	22833.838995	30.425780
468.188215	22874.179801	30.430797
468.273419	22909.947144	30.435815
468.903307	22945.092184	30.440832
469.099549	22988.541393	30.445850
469.740734	23028.181582	30.450868
470.318942	23062.631732	30.455885
470.348999	23104.181101	30.460903
471.408370	23136.747062	30.465920
471.768863	23186.887105	30.470938
472.251760	23212.060600	30.475956
472.596410	23259.666302	30.480973
472.932264	23298.996629	30.485991
473.873730	23321.966579	30.491008
473.803819	23386.591919	30.496026
474.633756	23414.356273	30.501044
474.952295	23452.768938	30.506061
475.254737	23488.411602	30.511079
475.864640	23535.989263	30.516096
476.219161	23579.766968	30.521114
476.811668	23620.993351	30.526132
477.092601	23671.330339	30.531149
477.339878	23718.340885	30.536167
478.102715	23744.718343	30.541184
478.316647	23800.893816	30.546202
478.815678	23837.464577	30.551220
479.754598	23873.617967	30.556237
480.463716	23912.268847	30.561255
480.786863	23947.427951	30.566272
481.228676	23982.429590	30.571290
482.036344	24013.759785	30.576308
482.309787	24056.327610	30.581325
482.781161	24074.945797	30.586343
483.712060	24091.195395	30.591360
484.231435	24121.665856	30.596378
484.670126	24148.453248	30.601396
485.093382	24176.404245	30.606413
485.468147	24209.304398	30.611431
485.715777	24234.200328	30.616448
486.210934	24263.720198	30.621466
486.974465	24286.655302	30.626484
487.618719	24310.054507	30.631501
487.849758	24358.860031	30.636519
488.283345	24381.052226	30.641536
488.516639	24411.008737	30.646554
488.987514	24445.850794	30.651572
489.776556	24475.225773	30.656589
489.667483	24520.776696	30.661607
490.312362	24546.335338	30.666624
490.789743	24587.382477	30.671642
491.249987	24624.146343	30.676660
491.663235	24667.295361	30.681677
491.585717	24716.893187	30.686695
492.657801	24755.775035	30.691712
492.838733	24803.342103	30.696730
493.514294	24857.758816	30.701748
494.152632	24903.136620	30.706765
494.089853	24954.478501	30.711783
494.645408	24994.405855	30.716800
495.211422	25048.123015	30.721818
495.830081	25088.756629	30.726836
496.048015	25146.947360	30.731853
496.506119	25195.627883	30.736871
497.269707	25243.265721	30.741888
497.810223	25286.860921	30.746906
498.243404	25328.860759	30.751924
499.169429	25384.769228	30.756941
499.655888	25430.635149	30.761959
500.097560	25465.953599	30.766976
500.785956	25510.245098	30.771994
501.657561	25546.144374	30.777012
502.334302	25572.913567	30.782029
502.647192	25614.439371	30.787047
503.651468	25638.891599	30.792064
504.001990	25672.181490	30.797082
504.746797	25696.479767	30.802100
505.536443	25725.088064	30.807117
505.824066	25746.870543	30.812135
506.245452	25780.233665	30.817152
506.800469	25803.150600	30.822170
507.352409	25820.855174	30.827188
507.642542	25848.102372	30.832205
508.041122	25892.565568	30.837223
508.587046	25913.219169	30.842240
509.089821	25941.829434	30.847258
509.224042	25971.916514	30.852276
509.826806	25997.222636	30.857293
509.995348	26029.027297	30.862311
510.516398	26056.509072	30.867328
510.715523	26096.932400	30.872346
510.916399	26132.850025	30.877364
511.582909	26171.490315	30.882381
511.717462	26223.309018	30.887399
512.384121	26258.642220	30.892416
512.981297	26309.108082	30.897434
513.242411	26356.263610	30.902452
513.965281	26407.089490	30.907469
514.151490	26460.299125	30.912487
514.596499	26500.518853	30.917504
515.116359	26558.852528	30.922522
515.448332	26606.094403	30.927540
516.341626	26647.569025	30.932557
516.718639	26704.376296	30.937575
517.588804	26745.710681	30.942592
518.132203	26801.126450	30.947610
518.668031	26845.787863	30.952628
519.609694	26885.021046	30.957645
520.082466	26930.753189	30.962663
520.743621	26975.111369	30.967680
521.192271	27020.348107	30.972698
521.895699	27056.858996	30.977716
522.402039	27090.029306	30.982733
522.661361	27129.433227	30.987751
523.076043	27180.450878	30.992768
523.452860	27224.002561	30.997786
523.766901	27275.600658	31.002804
524.205717	27329.578912	31.007821
524.759121	27382.231217	31.012839
525.100221	27424.947676	31.017856
525.775602	27473.728118	31.022874
525.962453	27535.258863	31.027892
526.964120	27582.465466	31.032909
527.035404	27657.306748	31.037927
527.547987	27695.871210	31.042944
528.711396	27746.287618	31.047962
529.440381	27791.072153	31.052980
530.181267	27832.036754	31.057997
530.698296	27890.438720	31.063015
531.406112	27930.880945	31.068032
531.825349	27973.807019	31.073050
532.020156	28021.445981	31.078068
532.900284	28064.519498	31.083085
533.029811	28115.349142	31.088103
533.621322	28152.318414	31.093120
534.305987	28198.218944	31.098138
534.552909	28252.126832	31.103156
535.225064	28296.609801	31.108173
535.675731	28343.811842	31.113191
536.426888	28390.268054	31.118208
536.690278	28438.994110	31.123226
537.292796	28479.692432	31.128244
538.479951	28513.411202	31.133261
538.783014	28552.676092	31.138279
539.371695	28582.240214	31.143296
539.554801	28618.601127	31.148314
540.577183	28654.965544	31.153332
541.481222	28674.869898	31.158349
541.570453	28712.657964	31.163367
541.951428	28755.554380	31.168384
542.355232	28794.745500	31.173402
542.676732	28841.911254	31.178420
543.404832	28871.485215	31.183437
543.866430	28920.699615	31.188455
544.199669	28964.909035	31.193472
544.660698	29003.872493	31.198490
545.307505	29063.373752	31.203508
545.630571	29109.414825	31.208525
546.258820	29162.454968	31.213543
546.735292	29207.679193	31.218560
547.619393	29259.093511	31.223578
547.816190	29313.641697	31.228596
548.596430	29355.053022	31.233613
549.107098	29413.946867	31.238631
549.426772	29464.526650	31.243648
550.005840	29516.759433	31.248666
550.737999	29568.659111	31.253684
551.552017	29621.920163	31.258701
551.590039	29668.750498	31.263719
552.397425	29727.126996	31.268736
553.004127	29769.630803	31.273754
553.327191	29825.590007	31.278772
554.468356	29871.772423	31.283789
554.958483	29916.118608	31.288807
555.208279	29961.417274	31.293824
555.983725	30013.250007	31.298842
556.155543	30061.196458	31.303860
556.801634	30105.196807	31.308877
557.303440	30166.452500	31.313895
557.995952	30217.339291	31.318912
558.585209	30270.873087	31.323930
558.767864	30324.642032	31.328948
559.578828	30378.285864	31.333965
559.897412	30428.088657	31.338983
560.651865	30487.065743	31.344000
561.479456	30533.449702	31.349018
561.995135	30589.157037	31.354036
562.733169	30634.734417	31.359053
563.111978	30683.485037	31.364071
563.786050	30730.237589	31.369088
564.716552	30774.538026	31.374106
564.967567	30824.816155	31.379124
565.695548	30866.501269	31.384141
566.439228	30911.585205	31.389159
566.979604	30955.850550	31.394176
567.515928	30994.521490	31.399194
567.890671	31034.630448	31.404212
568.771780	31063.006666	31.409229
569.468724	31109.127790	31.414247
570.160454	31128.559888	31.419264
570.415761	31169.263480	31.424282
571.165791	31205.386969	31.429300
571.430681	31244.547772	31.434317
571.926132	31276.606151	31.439335
572.384727	31322.502621	31.444352
573.033760	31362.790931	31.449370
573.310053	31414.332477	31.454388
573.739940	31451.842491	31.459405
574.412973	31508.905439	31.464423
574.834488	31548.604708	31.469440
575.753379	31600.116996	31.474458
575.622247	31650.594062	31.479476
576.514143	31716.452561	31.484493
577.151790	31775.878450	31.489511
577.333263	31822.217646	31.494528
577.848200	31875.445396	31.499546
577.785579	31949.996639	31.504564
578.602454	32006.609678	31.509581
579.151008	32084.279639	31.514599
579.619325	32155.643697	31.519616
580.294164	32211.873397	31.524634
580.706517	32282.165628	31.529652
581.605656	32354.406091	31.534669
582.467615	32417.501140	31.539687
583.013778	32473.492145	31.544704
583.882764	32527.192076	31.549722
584.602867	32589.629435	31.554740
585.424971	32633.444596	31.559757
585.681046	32695.894784	31.564775
586.469565	32746.742592	31.569792
587.636026	32797.680111	31.574810
587.980878	32851.045280	31.579828
588.883436	32899.649688	31.584845
589.587423	32937.740484	31.589863
590.193077	32994.463060	31.594880
590.909837	33032.364461	31.599898
591.327170	33082.810563	31.604916
592.136658	33120.476716	31.609933
592.142453	33169.212124	31.614951
592.709612	33223.730051	31.619968
593.567235	33269.415483	31.624986
593.560469	33326.681252	31.630004
594.268044	33374.203645	31.635021
594.788569	33439.462948	31.640039
595.589501	33492.596761	31.645056
596.345719	33546.757762	31.650074
596.932903	33604.330289	31.655092
597.324907	33646.845206	31.660109
598.042831	33694.784605	31.665127
598.199224	33753.843404	31.670144
598.983154	33789.519470	31.675162
599.456315	33858.607509	31.680180
600.143520	33904.914552	31.685197
600.962944	33956.033866	31.690215
601.427623	33991.025036	31.695232
602.503701	34040.087534	31.700250
602.934579	34078.104642	31.705268
603.673569	34117.037526	31.710285
604.553658	34157.220190	31.715303
605.091129	34198.723371	31.720320
606.073603	34228.383140	31.725338
606.254370	34266.594998	31.730356
606.710012	34311.600100	31.735373
607.592029	34342.095810	31.740391
607.898027	34403.130415	31.745408
608.113826	34441.409610	31.750426
608.796341	34493.041074	31.755444
609.114481	34544.953004	31.760461
609.593215	34601.948784	31.765479
609.955919	34665.437728	31.770496
610.668972	34717.159611	31.775514
611.066518	34789.657667	31.780532
611.759269	34846.196130	31.785549
612.421057	34906.398715	31.790567
612.955329	34962.070523	31.795584
613.543379	35027.103013	31.800602
614.203170	35090.346047	31.805620
614.503005	35165.689522	31.810637
615.441048	35228.173035	31.815655
615.920233	35301.826925	31.820672
616.766903	35350.753253	31.825690
617.490361	35426.936941	31.830708
617.988198	35492.736033	31.835725
618.668445	35543.560770	31.840743
619.308273	35612.992133	31.845760
620.104715	35671.314133	31.850778
620.857956	35738.862902	31.855796
621.316037	35793.851197	31.860813
622.020382	35849.596621	31.865831
622.623974	35927.608417	31.870848
623.031867	35980.164783	31.875866
624.047065	36048.207542	31.880884
624.450805	36114.479690	31.885901
625.338830	36170.668333	31.890919
625.846073	36210.522748	31.895936
627.243897	36271.759222	31.900954
627.301447	36327.998656	31.905972
628.110214	36391.825145	31.910989
628.659678	36432.617757	31.916007
628.799779	36497.891254	31.921024
629.563837	36562.728245	31.926042
629.995791	36621.507326	31.931060
630.871621	36687.580426	31.936077
631.890116	36722.295198	31.941095
632.701301	36790.539002	31.946112
633.709149	36821.012903	31.951130
634.203264	36870.304106	31.956148
634.707973	36906.635166	31.961165
635.800684	36946.377601	31.966183
635.966165	36987.425059	31.971200
636.408741	37025.819096	31.976218
636.966189	37073.730680	31.981236
637.513690	37121.264003	31.986253
638.170704	37173.458055	31.991271
638.632081	37219.843352	31.996288
639.572624	37272.014634	32.001306
639.982856	37319.877832	32.006324
640.431566	37376.813716	32.011341
640.922246	37427.641233	32.016359
641.278327	37484.623765	32.021376
641.811548	37545.789708	32.026394
642.372555	37606.268724	32.031412
643.149416	37664.813620	32.036429
643.716864	37742.122164	32.041447
644.259857	37803.331632	32.046464
644.853593	37881.611057	32.051482
645.524928	37937.508987	32.056500
646.138447	38022.909716	32.061517
647.226962	38071.630440	32.066535
647.623062	38155.779814	32.071552
648.494685	38213.579895	32.076570
649.068317	38276.612113	32.081588
649.648577	38350.622748	32.086605
650.406226	38414.239550	32.091623
650.714033	38475.797951	32.096640
651.520560	38540.161157	32.101658
652.074146	38611.952293	32.106676
652.709350	38701.019095	32.111693
653.312134	38762.563102	32.116711
653.940111	38841.573157	32.121728
654.497271	38906.731192	32.126746
655.648128	38981.642405	32.131764
656.240943	39049.040751	32.136781
656.871254	39114.648379	32.141799
657.304640	39203.551263	32.146816
658.043673	39265.157392	32.151834
659.146672	39345.869722	32.156852
659.708934	39407.042483	32.161869
660.531970	39468.117173	32.166887
661.095650	39530.242599	32.171904
661.507679	39599.602045	32.176922
662.320253	39664.801158	32.181940
662.875966	39731.593115	32.186957
663.986357	39794.370453	32.191975
664.569153	39867.119430	32.196992
665.862900	39922.875906	32.202010
666.305337	39980.190523	32.207028
666.729779	40046.225601	32.212045
667.428428	40099.866522	32.217063
667.310955	40156.126009	32.222080
668.317090	40224.229595	32.227098
669.334585	40278.224012	32.232116
669.516013	40344.642717	32.237133
670.583277	40404.849229	32.242151
671.029296	40452.434849	32.247168
671.802878	40517.457343	32.252186
672.571257	40567.496229	32.257204
673.527331	40624.961467	32.262221
674.462124	40667.076494	32.267239
675.024691	40729.130762	32.272256
675.593502	40766.891815	32.277274
676.332038	40807.158627	32.282292
676.667988	40873.785026	32.287309
677.210476	40921.145267	32.292327
678.413291	40974.528877	32.297344
679.022322	41045.966593	32.302362
679.670874	41084.113065	32.307380
679.949550	41151.594960	32.312397
680.978792	41200.916030	32.317415
681.492079	41280.800937	32.322432
681.798237	41337.564590	32.327450
682.522710	41397.958498	32.332468
683.013443	41475.548520	32.337485
684.012273	41530.798917	32.342503
684.149083	41599.939026	32.347520
684.863483	41670.668640	32.352538
685.529422	41746.200677	32.357556
685.831352	41820.516692	32.362573
687.071737	41889.441247	32.367591
687.940010	41978.085841	32.372608
688.605585	42044.301551	32.377626
689.522763	42102.765225	32.382644
690.025447	42164.764819	32.387661
691.048780	42232.438355	32.392679
691.703219	42299.476940	32.397696
692.354514	42355.826249	32.402714
693.517048	42411.100728	32.407732
694.374967	42487.677926	32.412749
695.250941	42519.593067	32.417767
695.922137	42597.140481	32.422784
696.342854	42647.338569	32.427802
697.381440	42691.359911	32.432820
697.810576	42756.016722	32.437837
698.352798	42805.776389	32.442855
699.344599	42862.584156	32.447872
699.779319	42926.830641	32.452890
700.361746	42976.902998	32.457908
700.927025	43044.923933	32.462925
701.605685	43105.025138	32.467943
702.452932	43173.121554	32.472960
702.791513	43226.602443	32.477978
703.867577	43290.596753	32.482996
704.851301	43343.631450	32.488013
705.630832	43406.143460	32.493031
706.370220	43458.371997	32.498048
706.752664	43514.051809	32.503066
707.587156	43563.804979	32.508084
707.791911	43622.806782	32.513101
708.367155	43680.109422	32.518119
709.045957	43740.058234	32.523136
709.518705	43812.907657	32.528154
710.723698	43862.217835	32.533172
711.158449	43933.281997	32.538189
711.492887	43995.551532	32.543207
711.854267	44065.236721	32.548224
712.483276	44135.106716	32.553242
713.480408	44197.612172	32.558260
713.769373	44284.881275	32.563277
714.355259	44352.695845	32.568295
714.975944	44436.433266	32.573312
715.789563	44525.317279	32.578330
716.884479	44604.210060	32.583348
717.466982	44689.541611	32.588365
718.101690	44753.292951	32.593383
719.231705	44843.355419	32.598400
719.846468	44910.747977	32.603418
721.134953	44982.134788	32.608436
721.191231	45072.561825	32.613453
722.324080	45138.582459	32.618471
723.169834	45212.867433	32.623488
723.402340	45303.463207	32.628506
723.963681	45373.285838	32.633524
724.787980	45447.934883	32.638541
725.326204	45531.144884	32.643559
726.225800	45614.799383	32.648576
727.027442	45692.876171	32.653594
728.149401	45781.042329	32.658612
728.380881	45859.605000	32.663629
729.274294	45950.187238	32.668647
730.241595	46021.604191	32.673664
730.594313	46102.647405	32.678682
731.521466	46188.521383	32.683700
732.385958	46271.004622	32.688717
733.122779	46345.920667	32.693735
733.776915	46430.460534	32.698752
734.938357	46508.997953	32.703770
736.270980	46562.608459	32.708788
737.442140	46625.836350	32.713805
738.375443	46691.336157	32.718823
739.387642	46750.500774	32.723840
739.707799	46806.077939	32.728858
740.357434	46865.325902	32.733876
741.297359	46936.290284	32.738893
741.878222	46980.370114	32.743911
742.493161	47048.906725	32.748928
742.829984	47115.121482	32.753946
743.631916	47171.891492	32.758964
744.023242	47252.028310	32.763981
744.787061	47328.824752	32.768999
745.422440	47388.682548	32.774016
745.904863	47463.795302	32.779034
746.561009	47519.415886	32.784052
747.085209	47595.570097	32.789069
748.185315	47658.355496	32.794087
749.280144	47714.922864	32.799104
750.206109	47797.242549	32.804122
751.034963	47850.410246	32.809140
751.402672	47913.786444	32.814157
751.767902	47984.013520	32.819175
752.749168	48046.907570	32.824192
752.874100	48123.055039	32.829210
753.865446	48213.993043	32.834228
754.149933	48290.270443	32.839245
755.160261	48354.937453	32.844263
756.109039	48446.063283	32.849280
756.468754	48533.329581	32.854298
757.653591	48602.721816	32.859316
758.646333	48679.228932	32.864333
759.243465	48757.553803	32.869351
760.473898	48821.619492	32.874368
761.257168	48900.032114	32.879386
762.027314	48970.498410	32.884404
762.960778	49033.558194	32.889421
763.263411	49112.073507	32.894439
764.458380	49176.108256	32.899456
764.701285	49260.989029	32.904474
765.837737	49332.042185	32.909492
766.202318	49417.551229	32.914509
766.911569	49493.715685	32.919527
767.716010	49563.623483	32.924544
768.323431	49665.403346	32.929562
769.249854	49746.009015	32.934580
770.026659	49823.167625	32.939597
770.633525	49908.482669	32.944615
771.701228	49994.071891	32.949632
772.463622	50078.858080	32.954650
773.386571	50140.645394	32.959668
774.389676	50226.391177	32.964685
774.942049	50303.972590	32.969703
776.175998	50369.750562	32.974720
776.946901	50447.253631	32.979738
777.840071	50520.180604	32.984756
778.579686	50601.176474	32.989773
778.940436	50669.041678	32.994791
779.757558	50735.322850	32.999808
780.370930	50817.043542	33.004826
781.017016	50884.469661	33.009844
781.755313	50973.060420	33.014861
782.265504	51069.438796	33.019879
783.339301	51144.709634	33.024896
784.019597	51231.483632	33.029914
784.994608	51317.232798	33.034932
786.084555	51387.869173	33.039949
786.807420	51465.857683	33.044967
787.793654	51547.629651	33.049984
788.282463	51621.992007	33.055002
789.702749	51679.757327	33.060020
790.526438	51738.053326	33.065037
791.028112	51806.553689	33.070055
791.901714	51872.773263	33.075072
792.538070	51930.282291	33.080090
793.195766	52004.966510	33.085108
793.790399	52075.580280	33.090125
794.498817	52142.111184	33.095143
795.774247	52197.306930	33.100160
796.260703	52288.898356	33.105178
796.805203	52351.334250	33.110196
797.502785	52431.833767	33.115213
798.226561	52511.019673	33.120231
799.390183	52569.213757	33.125248
799.937871	52659.639007	33.130266
800.784073	52732.194221	33.135284
801.639882	52803.198506	33.140301
802.264626	52887.041430	33.145319
803.158885	52969.734009	33.150336
803.548787	53048.621914	33.155354
804.669551	53139.027779	33.160372
805.143592	53220.399637	33.165389
805.780481	53316.192245	33.170407
806.459171	53408.686685	33.175424
807.469457	53500.049356	33.180442
807.993913	53594.788183	33.185460
808.991113	53683.098528	33.190477
809.928946	53789.580476	33.195495
811.000365	53865.102927	33.200512
811.622165	53962.763610	33.205530
812.480909	54044.289403	33.210548
813.704030	54125.792286	33.215565
814.050535	54230.259283	33.220583
815.466977	54304.806965	33.225600
815.925070	54410.409340	33.230618
816.173366	54487.918238	33.235636
817.261157	54580.801742	33.240653
818.085246	54689.519764	33.245671
819.367442	54768.247851	33.250688
819.988741	54865.496785	33.255706
821.028571	54938.879107	33.260724
822.055351	55022.762581	33.265741
822.854585	55119.053353	33.270759
824.076599	55191.864761	33.275776
825.072973	55276.054116	33.280794
826.229273	55345.098117	33.285812
827.319880	55422.707350	33.290829
827.648677	55485.365108	33.295847
828.654118	55567.000622	33.300864
829.394813	55643.113398	33.305882
829.965411	55713.893487	33.310900
830.981347	55788.940292	33.315917
831.688858	55880.072658	33.320935
832.533246	55945.184778	33.325952
833.287590	56024.175909	33.330970
833.492664	56101.619594	33.335988
834.549108	56174.758001	33.341005
835.116202	56260.169266	33.346023
835.843684	56317.365138	33.351040
836.421954	56413.088609	33.356058
837.162156	56488.781954	33.361076
838.264561	56574.658770	33.366093
838.950470	56660.826411	33.371111
839.558064	56747.426784	33.376128
840.390134	56832.520726	33.381146
840.913813	56924.328369	33.386164
842.100534	57021.786011	33.391181
842.379549	57112.269737	33.396199
843.643206	57203.986256	33.401216
844.576507	57307.218767	33.406234
845.226255	57404.896485	33.411252
846.301012	57496.249897	33.416269
847.117262	57601.049608	33.421287
847.904642	57699.458348	33.426304
849.026847	57770.957280	33.431322
850.157825	57853.321703	33.436340
851.366540	57934.303950	33.441357
852.383104	58038.379700	33.446375
853.426806	58113.731480	33.451392
854.006464	58204.387376	33.456410
854.913030	58287.575569	33.461428
855.860547	58368.159283	33.466445
856.673664	58456.136718	33.471463
857.513225	58541.821405	33.476480
858.354169	58635.942295	33.481498
858.935705	58712.645566	33.486516
860.065101	58799.399809	33.491533
860.247742	58903.483675	33.496551
860.713926	58996.482062	33.501568
861.783299	59086.290792	33.506586
862.508093	59199.184066	33.511604
863.868731	59281.717187	33.516621
864.677271	59400.237300	33.521639
865.639166	59483.298899	33.526656
866.411381	59591.245761	33.531674
866.984547	59677.593749	33.536692
867.899112	59785.957957	33.541709
868.909108	59879.142574	33.546727
869.560168	59971.320725	33.551744
870.623035	60078.532669	33.556762
871.361947	60181.262671	33.561780
872.295018	60271.543993	33.566797
873.340016	60382.956805	33.571815
874.384323	60473.139301	33.576832
875.479941	60573.516022	33.581850
876.290077	60665.590176	33.586868
877.479115	60759.432708	33.591885
877.920319	60848.898338	33.596903
879.110763	60939.394522	33.601920
879.712669	61021.920291	33.606938
880.420869	61123.589910	33.611956
881.546215	61192.010161	33.616973
882.205888	61283.006113	33.621991
882.698762	61369.137837	33.627008
884.228299	61461.126665	33.632026
884.600359	61551.364476	33.637044
885.477354	61641.926550	33.642061
886.132373	61749.917100	33.647079
887.041523	61828.930333	33.652096
887.995140	61933.467221	33.657114
888.669999	62038.045890	33.662132
889.940446	62117.710177	33.667149
890.764692	62216.417848	33.672167
891.764470	62308.649846	33.677184
893.298477	62400.225713	33.682202
894.302853	62487.380063	33.687220
895.681111	62546.834607	33.692237
896.947362	62629.864838	33.697255
898.188677	62697.438423	33.702272
899.460345	62760.532690	33.707290
900.227896	62821.995806	33.712308
901.093581	62884.652986	33.717325
902.034316	62950.655299	33.722343
902.667121	63023.076391	33.727360
903.536224	63091.727468	33.732378
903.808306	63172.518240	33.737396
904.853663	63237.961736	33.742413
905.471131	63321.256134	33.747431
906.650407	63393.768528	33.752448
907.654945	63462.257284	33.757466
908.355963	63547.187856	33.762484
909.247760	63629.202006	33.767501
910.053572	63715.158803	33.772519
910.554386	63803.681494	33.777536
911.603779	63882.914672	33.782554
912.322435	63980.173495	33.787572
913.145161	64069.025165	33.792589
913.698320	64170.543153	33.797607
914.336303	64273.611462	33.802624
915.231207	64372.663326	33.807642
915.715069	64483.807432	33.812660
916.968429	64595.966688	33.817677
918.019771	64705.158447	33.822695
918.680127	64810.288396	33.827712
919.990073	64914.181749	33.832730
920.866106	65013.397843	33.837748
921.895923	65114.371249	33.842765
922.844355	65219.122824	33.847783
923.445534	65325.998919	33.852800
924.563810	65434.824135	33.857818
925.254414	65538.159325	33.862836
926.407540	65623.320898	33.867853
927.687177	65733.616036	33.872871
928.551461	65832.752954	33.877888
929.833716	65930.443652	33.882906
930.759042	66020.121858	33.887924
931.807056	66109.755692	33.892941
932.438119	66188.149019	33.897959
932.987540	66289.274518	33.902976
934.194370	66368.748759	33.907994
934.486670	66461.764028	33.913012
935.743985	66557.689956	33.918029
936.274676	66659.960598	33.923047
937.016037	66755.255774	33.928064
938.124379	66855.161383	33.933082
939.004881	66964.528962	33.938100
940.419360	67060.280766	33.943117
941.472875	67172.060425	33.948135
942.231655	67270.128627	33.953152
943.154089	67365.568561	33.958170
943.760827	67471.615443	33.963188
944.669282	67578.341394	33.968205
945.789252	67688.609923	33.973223
946.185541	67793.864468	33.978240
947.173739	67902.462105	33.983258
948.080010	68024.308552	33.988276
948.857890	68140.585162	33.993293
949.868569	68261.620470	33.998311
950.425126	68386.133981	34.003328
951.709447	68505.200388	34.008346
952.211856	68629.989411	34.013364
953.608992	68762.780443	34.018381
954.882669	68888.111764	34.023399
955.635617	69016.830961	34.028416
956.712554	69134.215750	34.033434
957.885785	69259.369577	34.038452
959.177145	69368.508382	34.043469
960.240696	69489.492338	34.048487
961.056654	69608.917974	34.053504
962.363286	69707.979008	34.058522
963.386769	69825.894525	34.063540
964.242292	69941.171223	34.068557
965.369673	70041.102768	34.073575
966.470258	70158.104515	34.078592
967.345522	70257.755046	34.083610
968.097678	70391.512687	34.088628
968.973789	70484.940741	34.093645
970.129822	70604.109810	34.098663
970.659002	70726.879710	34.103680
972.189666	70828.077947	34.108698
973.057052	70947.162325	34.113716
973.668805	71056.999923	34.118733
974.902110	71176.893100	34.123751
976.338677	71276.358378	34.128768
977.778649	71377.504359	34.133786
978.772603	71490.784054	34.138804
979.941164	71580.575471	34.143821
981.270663	71676.274927	34.148839
981.547458	71781.822587	34.153856
982.790617	71874.510075	34.158874
983.720746	71964.954085	34.163892
984.700347	72047.997645	34.168909
985.342663	72138.886320	34.173927
985.856871	72225.574798	34.178944
986.997697	72329.604077	34.183962
987.856587	72427.637871	34.188980
988.871953	72524.712049	34.193997
989.947066	72627.950838	34.199015
990.572410	72732.203248	34.204032
991.512459	72849.846749	34.209050
992.352330	72950.097807	34.214068
993.223987	73072.227409	34.219085
994.176046	73169.226330	34.224103
995.118328	73298.404571	34.229120
995.868057	73398.924989	34.234138
996.802805	73538.298886	34.239156
997.760116	73649.694596	34.244173
999.476760	73752.843461	34.249191
1001.179591	73846.585523	34.254208
1002.960356	73936.941071	34.259226
1004.138052	74031.209898	34.264244
1004.958705	74121.662145	34.269261
1005.818649	74217.669691	34.274279
1006.314949	74306.215330	34.279296
1008.042182	74398.452053	34.284314
1008.999914	74501.283138	34.289332
1009.969950	74590.443499	34.294349
1011.073499	74686.825308	34.299367
1011.763368	74790.174455	34.304384
1012.568726	74895.199437	34.309402
1013.321924	74983.808304	34.314420
1014.137543	75098.716758	34.319437
1015.083092	75205.825535	34.324455
1016.105553	75312.322262	34.329472
1017.119671	75422.796068	34.334490
1018.746201	75517.828365	34.339508
1019.724938	75618.715284	34.344525
1021.152278	75696.981775	34.349543
1022.215188	75804.877693	34.354560
1023.473120	75904.305950	34.359578
1024.411443	76003.874019	34.364596
1025.224537	76099.164850	34.369613
1026.470023	76197.661158	34.374631
1027.442503	76301.301719	34.379648
1028.428579	76394.891589	34.384666
1029.038280	76492.776289	34.389684
1029.578885	76597.409808	34.394701
1030.939923	76697.571341	34.399719
1031.415402	76799.846166	34.404736
1032.768201	76909.420961	34.409754
1033.867519	77013.759175	34.414772
1034.681346	77131.593119	34.419789
1035.520022	77234.103086	34.424807
1036.340900	77359.249950	34.429824
1037.531122	77469.112757	34.434842
1038.770957	77561.479372	34.439860
1039.700289	77676.706676	34.444877
1041.060581	77761.426124	34.449895
1041.559591	77871.508496	34.454912
1042.635038	77966.254361	34.459930
1043.535071	78081.280022	34.464948
1044.259331	78187.984623	34.469965
1045.316446	78306.823237	34.474983
1046.015307	78424.126688	34.480000
1046.915453	78540.261042	34.485018
1048.179870	78661.862542	34.490036
1048.789993	78783.442418	34.495053
1050.020760	78903.356698	34.500071
1050.989378	79037.314332	34.505088
1052.213820	79173.046277	34.510106
1053.735522	79291.184581	34.515124
1054.592119	79415.105696	34.520141
1055.573664	79536.352806	34.525159
1056.250358	79663.774329	34.530176
1057.642940	79797.189052	34.535194
1058.748750	79925.511076	34.540212
1059.546729	80072.574912	34.545229
1060.761123	80183.358650	34.550247
1061.893179	80325.901969	34.555264
1063.168970	80467.089587	34.560282
1063.896797	80582.832985	34.565300
1065.180656	80724.849182	34.570317
1066.449992	80862.848167	34.575335
1067.201390	80986.314976	34.580352
1068.420419	81114.993000	34.585370
1069.450522	81253.993515	34.590388
1070.075579	81387.843987	34.595405
1071.201524	81529.859187	34.600423
1072.658226	81674.281916	34.605440
1073.484205	81805.732442	34.610458
1074.338943	81951.909152	34.615476
1075.384379	82093.801909	34.620493
1076.591360	82240.860253	34.625511
1077.611716	82390.395924	34.630528
1078.679289	82527.938570	34.635546
1080.182779	82671.684284	34.640564
1080.772162	82826.184896	34.645581
1082.308277	82959.609688	34.650599
1083.096678	83110.268468	34.655616
1084.102417	83254.128946	34.660634
1085.733173	83401.747598	34.665652
1086.713817	83550.172465	34.670669
1087.734209	83674.977955	34.675687
1088.833211	83828.918040	34.680704
1089.929253	83965.030356	34.685722
1091.271575	84096.413079	34.690740
1092.257776	84245.170715	34.695757
1093.693271	84383.033659	34.700775
1094.533207	84523.331596	34.705792
1095.594623	84675.393348	34.710810
1096.830760	84787.266504	34.715828
1097.737692	84915.404131	34.720845
1099.113302	85031.834065	34.725863
1099.984613	85163.728265	34.730880
1101.256253	85288.863703	34.735898
1102.535259	85403.477408	34.740916
1103.560945	85528.526915	34.745933
1104.836754	85644.919173	34.750951
1105.987298	85765.663244	34.755968
1107.104877	85887.987677	34.760986
1108.816758	85996.889259	34.766004
1110.009505	86117.015269	34.771021
1111.470020	86214.177998	34.776039
1112.737471	86323.506026	34.781056
1114.560361	86413.201282	34.786074
1116.079828	86507.346131	34.791092
1116.770527	86606.637537	34.796109
1117.743952	86700.629795	34.801127
1119.210572	86789.295687	34.806144
1119.918504	86897.242301	34.811162
1121.328506	86978.677765	34.816180
1122.091041	87088.899392	34.821197
1123.057549	87194.055700	34.826215
1123.798281	87301.347814	34.831232
1124.619038	87419.535751	34.836250
1125.797357	87523.287786	34.841268
1126.785304	87653.699077	34.846285
1127.351935	87766.117981	34.851303
1128.384856	87891.686012	34.856320
1129.021778	88029.756398	34.861338
1130.238310	88156.947249	34.866356
1131.369882	88299.348313	34.871373
1132.731162	88435.567065	34.876391
1133.807787	88568.815478	34.881408
1134.695165	88700.943863	34.886426
1136.316473	88837.825741	34.891444
1137.446132	88969.563095	34.896461
1138.638052	89105.629596	34.901479
1140.062147	89241.103514	34.906496
1140.835980	89367.891245	34.911514
1142.011161	89490.903648	34.916532
1143.120429	89638.724144	34.921549
1144.225555	89771.741408	34.926567
1145.675020	89907.341920	34.931584
1146.515816	90039.447895	34.936602
1147.957366	90167.847965	34.941620
1148.868924	90313.136808	34.946637
1150.095598	90457.522714	34.951655
1151.324394	90596.229913	34.956672
1152.634819	90711.176709	34.961690
1153.994460	90852.097250	34.966708
1155.331723	90983.510171	34.971725
1156.362535	91100.223742	34.976743
1157.443237	91238.781467	34.981760
1158.454747	91364.910513	34.986778
1160.352856	91463.874005	34.991796
1161.540973	91578.737276	34.996813
1162.476407	91681.801442	35.001831
1163.918299	91785.759567	35.006848
1164.881633	91888.156164	35.011866
1166.180655	92003.838886	35.016884
1167.093557	92118.135225	35.021901
1167.941500	92239.640199	35.026919
1168.842121	92347.741293	35.031936
1169.752723	92473.620753	35.036954
1171.257604	92589.628005	35.041972
1172.026658	92727.068184	35.046989
1172.770583	92865.974299	35.052007
1173.814948	92992.164335	35.057024
1174.826453	93144.571679	35.062042
1175.976460	93275.186774	35.067060
1176.693608	93432.981349	35.072077
1177.964108	93580.897541	35.077095
1179.255914	93738.754711	35.082112
1180.201781	93898.831276	35.087130
1181.716776	94036.945272	35.092148
1182.784811	94203.728490	35.097165
1183.797206	94349.938673	35.102183
1185.379554	94511.442859	35.107200
1186.103447	94672.762107	35.112218
1187.564145	94825.602892	35.117236
1189.187568	94973.978232	35.122253
1190.410759	95131.084402	35.127271
1191.478002	95273.116919	35.132288
1193.171915	95428.973735	35.137306
1194.848116	95563.908618	35.142324
1195.799247	95714.957706	35.147341
1197.079550	95860.736592	35.152359
1198.224183	96001.053397	35.157376
1199.609937	96152.207104	35.162394
1200.912991	96290.887393	35.167412
1202.220620	96435.071482	35.172429
1203.613742	96574.510970	35.177447
1204.642115	96711.674963	35.182464
1205.895274	96850.303351	35.187482
1207.513188	96970.142659	35.192500
1209.436498	97090.383208	35.197517
1210.584090	97217.700317	35.202535
1212.522384	97327.722796	35.207552
1213.514135	97455.306415	35.212570
1214.942281	97568.561695	35.217588
1215.737979	97685.309053	35.222605
1217.070371	97807.108752	35.227623
1218.329003	97917.767245	35.232640
1218.839255	98043.026646	35.237658
1220.376910	98160.556832	35.242676
1220.960027	98289.658864	35.247693
1221.750425	98433.121723	35.252711
1223.207083	98558.575109	35.257728
1224.353671	98698.161696	35.262746
1225.070336	98819.893864	35.267764
1226.120053	98951.690215	35.272781
1226.841605	99079.072777	35.277799
1228.105793	99226.786469	35.282816
1228.779242	99368.711035	35.287834
1229.974470	99520.360238	35.292852
1230.780618	99682.891403	35.297869
1231.425684	99836.800303	35.302887
1232.717777	100003.153896	35.307904
1233.621357	100177.036429	35.312922
1235.188263	100347.385495	35.317940
1236.020290	100520.434144	35.322957
1237.191329	100699.529643	35.327975
1238.443536	100882.947812	35.332992
1239.426218	101073.648758	35.338010
1241.080986	101244.483970	35.343028
1242.838474	101416.189946	35.348045
1244.089761	101603.574914	35.353063
1245.238233	101778.487178	35.358080
1246.809985	101943.582656	35.363098
1248.471946	102128.508393	35.368116
1249.842076	102296.125173	35.373133
1251.332877	102455.422003	35.378151
1252.938291	102623.035355	35.383168
1253.907272	102787.485936	35.388186
1255.226332	102949.363527	35.393204
1257.091829	103112.351334	35.398221
1258.341572	103270.008792	35.403239
1260.073824	103425.053079	35.408256
1261.032354	103586.796202	35.413274
1262.250649	103740.620698	35.418292
1263.579369	103903.522125	35.423309
1264.734389	104053.270759	35.428327
1266.500662	104202.859885	35.433344
1268.185589	104359.601127	35.438362
1269.823852	104489.575940	35.443380
1270.915464	104628.662518	35.448397
1272.114629	104784.914247	35.453415
1273.501047	104931.980070	35.458432
1274.456641	105072.248958	35.463450
1275.967015	105208.551138	35.468468
1276.925817	105363.243775	35.473485
1277.752740	105509.079448	35.478503
1279.572232	105655.327794	35.483520
1280.552538	105818.474930	35.488538
1282.318433	105945.994562	35.493556
1283.600092	106100.406485	35.498573
1284.312592	106250.112704	35.503591
1285.677575	106401.291997	35.508608
1286.880475	106565.149294	35.513626
1288.008676	106716.115056	35.518644
1289.423689	106863.605914	35.523661
1290.511858	107028.054202	35.528679
1292.240230	107168.535293	35.533696
1293.496075	107319.978208	35.538714
1294.764856	107466.749181	35.543732
1296.289744	107600.069009	35.548749
1297.136303	107730.022716	35.553767
1298.751279	107864.171452	35.558784
1299.887152	108001.814851	35.563802
1300.898558	108146.048549	35.568820
1302.148336	108279.485473	35.573837
1302.988746	108438.697801	35.578855
1304.490741	108573.931747	35.583872
1305.260293	108747.347729	35.588890
1306.504661	108897.125034	35.593908
1307.705830	109058.948756	35.598925
1308.685477	109227.796535	35.603943
1309.807276	109392.496018	35.608960
1311.147171	109579.011693	35.613978
1312.499262	109742.721159	35.618996
1313.580431	109931.761862	35.624013
1314.957725	110111.376287	35.629031
1316.223101	110289.117211	35.634048
1317.517313	110475.374778	35.639066
1318.537978	110664.829513	35.644084
1320.418905	110850.610535	35.649101
1321.711644	111036.682680	35.654119
1322.719129	111228.144101	35.659136
1324.290734	111403.040179	35.664154
1325.663019	111596.022645	35.669172
1327.393187	111775.529792	35.674189
1328.340707	111964.721246	35.679207
1330.207978	112149.051909	35.684224
1331.533581	112330.849292	35.689242
1333.060652	112506.285635	35.694260
1334.728930	112685.897817	35.699277
1335.810137	112878.917509	35.704295
1337.419334	113038.119633	35.709312
1338.744627	113223.614236	35.714330
1339.959257	113400.328310	35.719348
1341.922473	113564.453341	35.724365
1343.199900	113751.706708	35.729383
1344.734601	113912.072075	35.734400
1346.206965	114087.376258	35.739418
1347.193559	114258.612205	35.744436
1348.836324	114418.134289	35.749453
1350.305624	114588.833607	35.754471
1351.866460	114758.829461	35.759488
1353.718801	114907.900656	35.764506
1355.221646	115061.421983	35.769524
1357.161415	115211.715616	35.774541
1358.228778	115354.551528	35.779559
1359.914437	115505.855946	35.784576
1361.719448	115636.078624	35.789594
1362.704373	115787.040248	35.794612
1364.680780	115902.504433	35.799629
1366.081315	116039.080340	35.804647
1367.249573	116176.459978	35.809664
1368.647023	116303.458594	35.814682
1369.647191	116425.816808	35.819700
1370.783713	116546.070922	35.824717
1371.488441	116681.640203	35.829735
1372.629555	116816.096163	35.834752
1373.649700	116941.176177	35.839770
1374.492142	117099.329072	35.844788
1376.091160	117246.117906	35.849805
1377.068801	117403.320451	35.854823
1378.318929	117565.989147	35.859840
1379.735789	117714.113913	35.864858
1381.093362	117873.152106	35.869876
1382.605550	118022.339881	35.874893
1383.478768	118204.821141	35.879911
1384.615986	118365.239718	35.884928
1386.027450	118540.919767	35.889946
1386.996207	118732.843008	35.894964
1388.569145	118898.254819	35.899981
1389.668268	119095.333208	35.904999
1391.047373	119282.212025	35.910016
1392.354385	119467.697921	35.915034
1393.498286	119675.930693	35.920052
1395.289751	119867.193319	35.925069
1396.399916	120069.393702	35.930087
1397.691940	120252.810587	35.935104
1399.286120	120449.035317	35.940122
1401.004217	120657.716561	35.945140
1402.404697	120849.086485	35.950157
1403.228468	121047.033877	35.955175
1404.757173	121261.753173	35.960192
1406.211322	121456.424545	35.965210
1407.847606	121672.333269	35.970228
1409.578982	121865.431109	35.975245
1411.034000	122076.280488	35.980263
1412.612229	122255.904206	35.985280
1414.611632	122452.725379	35.990298
1416.068218	122645.125295	35.995316
1417.738706	122831.172399	36.000333
1419.132961	123021.697744	36.005351
1420.823932	123199.777352	36.010368
1422.465742	123390.823293	36.015386
1423.630455	123572.320174	36.020404
1425.513830	123749.346915	36.025421
1426.655725	123941.210861	36.030439
1428.176243	124122.148272	36.035456
1430.008736	124296.159446	36.040474
1431.696388	124458.972225	36.045492
1433.826584	124622.247664	36.050509
1435.384483	124772.796363	36.055527
1436.782345	124933.910062	36.060544
1438.270253	125087.334322	36.065562
1439.318002	125255.370983	36.070580
1440.667135	125402.080294	36.075597
1441.984506	125567.707327	36.080615
1443.431626	125739.496306	36.085632
1444.945646	125892.034275	36.090650
1446.005572	126046.684683	36.095668
1447.021757	126205.434469	36.100685
1448.262810	126366.150898	36.105703
1449.460859	126527.989845	36.110720
1450.525643	126698.971569	36.115738
1451.955525	126863.448520	36.120756
1453.343412	127023.790789	36.125773
1454.512483	127208.465592	36.130791
1455.387317	127399.268973	36.135808
1457.302450	127579.279951	36.140826
1458.596724	127775.821227	36.145844
1459.760621	127952.242269	36.150861
1461.320413	128164.477959	36.155879
1462.001216	128365.111399	36.160896
1463.632387	128558.805013	36.165914
1464.900097	128779.528994	36.170932
1466.424614	129000.530639	36.175949
1467.903678	129208.327793	36.180967
1469.360709	129417.814950	36.185984
1470.865018	129630.957482	36.191002
1472.306323	129853.752763	36.196020
1473.847375	130060.418871	36.201037
1475.312924	130298.784168	36.206055
1476.630550	130507.516145	36.211072
1478.667652	130726.536932	36.216090
1479.686827	130958.935447	36.221108
1481.655280	131163.856722	36.226125
1483.690358	131382.958953	36.231143
1484.948393	131606.228007	36.236160
1486.821607	131806.278534	36.241178
1488.481312	132013.852352	36.246196
1489.832541	132226.633416	36.251213
1491.369714	132438.271554	36.256231
1493.267865	132647.345203	36.261248
1494.421194	132854.600158	36.266266
1495.996874	133074.548649	36.271284
1497.538223	133276.246040	36.276301
1499.502387	133491.207175	36.281319
1500.797728	133687.447491	36.286336
1502.809438	133892.039431	36.291354
1504.247689	134086.447841	36.296372
1506.058271	134282.914462	36.301389
1507.749564	134467.287839	36.306407
1509.622686	134651.823574	36.311424
1510.883608	134849.357053	36.316442
1512.338867	135046.138739	36.321460
1514.020955	135242.720995	36.326477
1515.283471	135427.333333	36.331495
1516.530201	135637.127746	36.336512
1517.986158	135825.488004	36.341530
1519.242860	136032.660645	36.346548
1520.376092	136227.816134	36.351565
1521.937141	136443.686895	36.356583
1523.619630	136649.820522	36.361600
1524.771776	136856.204588	36.366618
1526.457894	137053.786811	36.371636
1528.302432	137223.567601	36.376653
1530.184376	137412.009771	36.381671
1531.298696	137591.793110	36.386688
1533.407943	137769.455251	36.391706
1534.816731	137954.288354	36.396724
1536.420627	138129.789896	36.401741
1537.935569	138307.549678	36.406759
1539.517306	138495.526858	36.411776
1541.060425	138683.549380	36.416794
1542.091770	138880.918321	36.421812
1543.601328	139057.606236	36.426829
1545.193819	139253.671886	36.431847
1546.464104	139455.011364	36.436864
1547.675858	139656.057334	36.441882
1548.999527	139854.349423	36.446900
1550.334997	140069.636051	36.451917
1551.504829	140289.449642	36.456935
1553.186591	140502.276375	36.461952
1554.720418	140724.557366	36.466970
1556.158841	140957.602554	36.471988
1557.550852	141182.570938	36.477005
1559.388380	141408.484139	36.482023
1560.465557	141652.428331	36.487040
1562.052403	141874.189674	36.492058
1563.669225	142122.766710	36.497076
1565.293558	142361.243062	36.502093
1566.862995	142586.447102	36.507111
1568.456418	142829.494828	36.512128
1570.717561	143054.338931	36.517146
1572.364771	143296.266427	36.522164
1573.930622	143520.818785	36.527181
1575.903954	143746.765671	36.532199
1577.214068	143985.988964	36.537216
1579.217743	144213.975126	36.542234
1580.863414	144435.377988	36.547252
1582.108023	144667.480756	36.552269
1583.996065	144890.255317	36.557287
1585.343752	145120.621219	36.562304
1587.522640	145336.710780	36.567322
1588.941418	145585.803398	36.572340
1590.392902	145797.194895	36.577357
1592.274464	146019.395424	36.582375
1594.101989	146243.824403	36.587392
1595.683448	146453.247553	36.592410
1597.126004	146682.646440	36.597428
1598.738667	146902.753621	36.602445
1600.304356	147121.843006	36.607463
1601.682313	147353.944390	36.612480
1603.417731	147579.918630	36.617498
1606.274293	147780.249081	36.622516
1607.937809	147969.564097	36.627533
1609.890628	148175.111245	36.632551
1611.479552	148398.439743	36.637568
1613.046104	148587.824521	36.642586
1614.508963	148769.962963	36.647604
1616.119212	148948.618186	36.652621
1617.744147	149124.977505	36.657639
1619.114750	149298.158173	36.662656
1620.644508	149479.922359	36.667674
1621.844672	149684.102763	36.672692
1623.052959	149883.465734	36.677709
1624.130238	150072.734083	36.682727
1625.403911	150292.005543	36.687744
1627.039140	150509.623665	36.692762
1628.104920	150736.296857	36.697780
1629.526109	150954.446366	36.702797
1631.177703	151189.701303	36.707815
1632.304948	151429.174240	36.712832
1634.010662	151674.033995	36.717850
1635.355562	151910.103476	36.722868
1636.685138	152185.606632	36.727885
1638.495585	152434.423700	36.732903
1640.203641	152685.211386	36.737920
1641.737012	152945.360163	36.742938
1643.062197	153202.716680	36.747956
1644.722131	153462.988856	36.752973
1647.103831	153724.644539	36.757991
1648.702775	153987.098565	36.763008
1650.991501	154224.061537	36.768026
1652.603295	154484.564822	36.773044
1654.359678	154745.896666	36.778061
1656.182031	154993.894018	36.783079
1657.717496	155251.182085	36.788096
1659.836022	155506.464887	36.793114
1661.305509	155752.292209	36.798132
1663.154736	156009.561536	36.803149
1664.994005	156262.650029	36.808167
1666.541834	156503.246208	36.813184
1668.098242	156753.923336	36.818202
1670.359506	156996.286314	36.823220
1672.514547	157244.538805	36.828237
1674.402290	157474.233526	36.833255
1676.154562	157702.404278	36.838272
1677.928366	157944.090491	36.843290
1679.708962	158178.638152	36.848308
1681.112410	158415.872177	36.853325
1683.070101	158644.447629	36.858343
1684.478178	158887.187553	36.863360
1685.969927	159120.925113	36.868378
1687.679644	159355.885032	36.873396
1688.716499	159609.163385	36.878413
1690.560930	159847.541761	36.883431
1692.405339	160087.240598	36.888448
1693.946171	160343.956886	36.893466
1695.907713	160592.555519	36.898484
1697.455705	160835.375383	36.903501
1699.263284	161084.306254	36.908519
1700.789510	161335.870600	36.913536
1702.558304	161568.870124	36.918554
1704.216386	161793.315812	36.923572
1705.447511	162042.218052	36.928589
1707.097092	162265.273019	36.933607
1708.720507	162498.720154	36.938624
1710.393222	162735.394922	36.943642
1712.508442	162963.415081	36.948660
1713.602259	163207.375690	36.953677
1715.661073	163431.831322	36.958695
1717.209552	163670.561090	36.963712
1718.796977	163918.861586	36.968730
1720.869409	164153.972868	36.973748
1722.235238	164405.317634	36.978765
1724.131674	164648.551625	36.983783
1725.938432	164898.079507	36.988800
1727.472109	165145.103148	36.993818
1729.121999	165412.390256	36.998836
1730.863290	165664.001034	37.003853
1732.277400	165901.574348	37.008871
1734.320612	166183.796166	37.013888
1735.977492	166437.518315	37.018906
1738.191197	166679.028311	37.023924
1739.860447	166951.485548	37.028941
1741.455849	167191.892063	37.033959
1743.255443	167465.131386	37.038976
1744.848791	167724.300948	37.043994
1747.186565	167980.018200	37.049012
1748.485231	168257.541152	37.054029
1750.466476	168504.414323	37.059047
1751.897493	168787.158657	37.064064
1753.628228	169045.287953	37.069082
1755.423518	169317.843587	37.074100
1757.037258	169594.983708	37.079117
1758.754920	169882.383836	37.084135
1760.688363	170135.236816	37.089152
1762.691597	170412.054562	37.094170
1764.502132	170671.069967	37.099188
1766.046494	170954.395636	37.104205
1768.374333	171226.398083	37.109223
1769.939005	171495.859704	37.114240
1771.776167	171760.827402	37.119258
1773.510487	172025.800521	37.124276
1775.424144	172296.518786	37.129293
1777.207837	172573.424667	37.134311
1779.019683	172838.885641	37.139328
1780.606737	173113.302069	37.144346
1782.188600	173385.640745	37.149364
1783.856998	173670.919741	37.154381
1786.163874	173939.658475	37.159399
1788.143367	174230.638757	37.164416
1789.949489	174486.939568	37.169434
1792.277390	174752.673775	37.174452
1793.666594	175020.981813	37.179469
1795.497019	175285.479107	37.184487
1797.659265	175551.701532	37.189504
1799.273780	175814.815647	37.194522
1800.945619	176060.947737	37.199540
1802.321199	176315.133591	37.204557
1803.728138	176546.150107	37.209575
1805.801784	176787.198805	37.214592
1807.318263	177057.466368	37.219610
1809.020695	177308.548891	37.224628
1810.734025	177566.228441	37.229645
1812.351911	177838.223082	37.234663
1814.237427	178105.736490	37.239680
1815.708859	178386.423268	37.244698
1817.356593	178647.596172	37.249716
1818.596362	178938.841197	37.254733
1820.492530	179217.804010	37.259751
1822.670677	179508.003160	37.264768
1824.486919	179803.387555	37.269786
1826.681724	180072.196466	37.274804
1828.561861	180360.672416	37.279821
1830.253083	180654.141266	37.284839
1831.951127	180936.064931	37.289856
1834.021313	181234.222875	37.294874
1835.820168	181541.865947	37.299892
1837.480723	181840.790916	37.304909
1839.580989	182143.416572	37.309927
1841.435177	182422.863515	37.314944
1843.174184	182724.675012	37.319962
1845.499399	183012.222335	37.324980
1847.187466	183302.105871	37.329997
1849.225099	183608.811888	37.335015
1851.389000	183887.064220	37.340032
1853.259895	184180.147411	37.345050
1855.192453	184475.912800	37.350068
1856.910173	184770.356497	37.355085
1858.747497	185064.529343	37.360103
1860.857966	185344.144213	37.365120
1862.482583	185653.759415	37.370138
1864.559444	185938.852382	37.375156
1866.403693	186235.810675	37.380173
1868.444891	186520.138855	37.385191
1870.379472	186811.959930	37.390208
1872.678175	187107.392393	37.395226
1874.936936	187386.666226	37.400244
1876.525555	187666.263829	37.405261
1878.492237	187956.437308	37.410279
1880.253444	188243.523440	37.415296
1881.673993	188531.426801	37.420314
1883.750315	188821.575526	37.425332
1886.004631	189103.525228	37.430349
1887.578116	189407.526320	37.435367
1889.595623	189687.105894	37.440384
1891.515647	189973.415864	37.445402
1893.501533	190262.940502	37.450420
1895.076239	190555.882480	37.455437
1896.923238	190840.648242	37.460455
1898.725302	191129.889980	37.465472
1900.401584	191428.785799	37.470490
1902.177163	191708.313938	37.475508
1903.698329	191985.828098	37.480525
1905.278386	192267.750990	37.485543
1907.348034	192549.902379	37.490560
1909.121444	192834.120303	37.495578
1911.474692	193113.539343	37.500596
1913.792474	193383.104354	37.505613
1916.016264	193655.972830	37.510631
1918.453634	193917.970315	37.515648
1919.859939	194193.205158	37.520666
1921.817332	194461.069017	37.525684
1923.599619	194729.660127	37.530701
1925.512626	195021.800616	37.535719
1927.323052	195306.508915	37.540736
1928.959954	195586.410698	37.545754
1931.368872	195875.050525	37.550772
1932.937367	196171.922902	37.555789
1934.526131	196459.338092	37.560807
1937.328737	196748.999151	37.565824
1939.270274	197031.322696	37.570842
1941.720671	197312.348542	37.575860
1944.159442	197579.225661	37.580877
1945.864765	197861.299227	37.585895
1947.572071	198136.037670	37.590912
1949.540919	198419.049712	37.595930
1951.356040	198710.921780	37.600948
1953.223951	198997.760720	37.605965
1954.565725	199284.621219	37.610983
1956.609215	199573.326598	37.616000
1958.276525	199887.669582	37.621018
1960.296718	200181.801804	37.626036
1962.151784	200487.690265	37.631053
1964.470259	200783.860066	37.636071
1966.624880	201091.735269	37.641088
1968.438688	201401.595657	37.646106
1970.127377	201692.539064	37.651124
1972.354751	202008.963169	37.656141
1974.387282	202313.475354	37.661159
1976.395778	202612.623603	37.666176
1978.517597	202926.188175	37.671194
1980.830086	203221.902198	37.676212
1983.430616	203503.354983	37.681229
1985.196700	203810.976706	37.686247
1987.354952	204100.791713	37.691264
1989.107218	204410.703747	37.696282
1990.985116	204702.026068	37.701300
1992.892369	205013.858926	37.706317
1994.259081	205329.815977	37.711335
1996.221025	205613.817647	37.716352
1997.843654	205938.001332	37.721370
2000.201135	206241.035556	37.726388
2002.417021	206561.332889	37.731405
2003.991346	206887.014667	37.736423
2006.058261	207201.436100	37.741440
2008.025217	207513.729634	37.746458
2010.032037	207808.766301	37.751476
2011.951865	208104.503721	37.756493
2013.755064	208406.494255	37.761511
2015.905493	208687.065628	37.766528
2017.226383	208999.164584	37.771546
2019.420675	209299.561349	37.776564
2021.387518	209597.367765	37.781581
2023.162765	209910.694105	37.786599
2025.275053	210231.192120	37.791616
2027.243742	210549.454784	37.796634
2029.131376	210877.520029	37.801652
2031.207177	211190.995454	37.806669
2032.584391	211517.964292	37.811687
2034.509710	211854.648797	37.816704
2036.420398	212199.805355	37.821722
2038.633479	212539.723229	37.826740
2040.372064	212891.499810	37.831757
2041.894797	213259.271169	37.836775
2044.252887	213602.650181	37.841792
2046.252708	213971.048063	37.846810
2048.487242	214342.457780	37.851828
2050.571549	214696.029963	37.856845
2052.625721	215073.452172	37.861863
2054.527034	215432.008717	37.866880
2056.805835	215800.308792	37.871898
2058.664321	216181.373884	37.876916
2060.705824	216542.592884	37.881933
2062.920602	216921.231260	37.886951
2065.347459	217282.875403	37.891968
2067.507626	217681.282384	37.896986
2069.694248	218040.289499	37.902004
2071.786244	218419.640951	37.907021
2074.056474	218782.053931	37.912039
2076.432295	219146.381893	37.917056
2078.831837	219509.831816	37.922074
2080.812819	219880.790386	37.927092
2083.197071	220248.791900	37.932109
2085.430885	220608.591338	37.937127
2087.705626	220971.433335	37.942144
2089.840017	221335.772219	37.947162
2091.880354	221697.067706	37.952180
2094.154997	222103.987556	37.957197
2095.491842	222473.270661	37.962215
2097.900533	222830.932329	37.967232
2099.888870	223204.356511	37.972250
2101.940122	223581.251630	37.977268
2104.431112	223937.533909	37.982285
2106.057868	224315.858481	37.987303
2108.240288	224679.176755	37.992320
2110.040927	225059.127927	37.997338
2112.280023	225428.560917	38.002356
2114.508658	225797.032173	38.007373
2116.981510	226178.062777	38.012391
2119.334011	226532.752958	38.017408
2121.590395	226891.878830	38.022426
2123.432187	227234.792889	38.027444
2125.750452	227566.534474	38.032461
2127.829848	227901.464401	38.037479
2130.027071	228229.824584	38.042496
2131.913029	228567.276625	38.047514
2133.795949	228909.378067	38.052532
2136.200535	229237.531335	38.057549
2138.428205	229582.501331	38.062567
2140.563319	229925.861908	38.067584
2143.080693	230253.366057	38.072602
2144.719577	230598.509491	38.077620
2146.791591	230940.741003	38.082637
2148.592530	231303.004635	38.087655
2150.620751	231656.674613	38.092672
2152.871018	232020.952348	38.097690
2154.632724	232380.280193	38.102708
2157.068429	232741.305733	38.107725
2158.803891	233121.111228	38.112743
2160.531988	233492.106214	38.117760
2162.746942	233871.406790	38.122778
2164.587625	234258.235273	38.127796
2167.052634	234647.074294	38.132813
2168.919194	235039.819494	38.137831
2170.836289	235435.453624	38.142848
2173.264357	235822.931436	38.147866
2175.422107	236229.858238	38.152884
2178.102926	236633.477989	38.157901
2179.869550	237049.715158	38.162919
2182.117268	237448.707844	38.167936
2184.226775	237856.435828	38.172954
2185.861358	238275.263921	38.177972
2188.322805	238690.177944	38.182989
2190.580476	239106.852972	38.188007
2192.485727	239524.728388	38.193024
2195.182131	239947.839172	38.198042
2197.378792	240377.101278	38.203060
2199.973407	240791.366727	38.208077
2202.606986	241203.595435	38.213095
2205.052805	241611.435718	38.218112
2207.426292	242012.608604	38.223130
2209.641783	242425.568117	38.228148
2212.522057	242815.233134	38.233165
2215.796001	243189.622125	38.238183
2218.622697	243566.851771	38.243200
2220.929180	243944.215804	38.248218
2223.110557	244317.282662	38.253236
2225.725580	244679.562739	38.258253
2227.645657	245058.947038	38.263271
2229.608906	245424.888546	38.268288
2231.926146	245792.527541	38.273306
2233.931308	246149.497816	38.278324
2236.385708	246517.142346	38.283341
2238.678348	246884.711860	38.288359
2240.903851	247248.965405	38.293376
2243.263944	247598.923073	38.298394
2244.990487	247947.889768	38.303412
2247.462502	248267.908652	38.308429
2249.424555	248614.883631	38.313447
2251.413310	248955.860430	38.318464
2253.466757	249293.347716	38.323482
2255.111602	249641.188094	38.328500
2257.253286	250003.378495	38.333517
2259.079355	250368.921943	38.338535
2261.256164	250733.064290	38.343552
2262.871941	251108.219099	38.348570
2264.668486	251499.857189	38.353588
2267.129419	251875.438485	38.358605
2269.610182	252276.114453	38.363623
2271.757578	252668.842567	38.368640
2274.174950	253059.953790	38.373658
2276.696716	253460.676637	38.378676
2278.956408	253846.784889	38.383693
2281.426165	254245.104418	38.388711
2283.799588	254643.643237	38.393728
2285.807070	255040.970751	38.398746
2287.824515	255448.915594	38.403764
2290.461300	255864.180504	38.408781
2292.485654	256268.036047	38.413799
2294.136259	256695.601224	38.418816
2296.651032	257115.688892	38.423834
2298.761648	257541.099719	38.428852
2301.095711	257978.516689	38.433869
2303.060446	258414.773678	38.438887
2305.128342	258857.518149	38.443904
2307.399295	259311.255953	38.448922
2309.333901	259767.664343	38.453940
2311.874405	260209.345451	38.458957
2314.090917	260676.913269	38.463975
2316.407903	261145.050179	38.468992
2319.314026	261598.259141	38.474010
2321.810999	262046.122813	38.479028
2324.595659	262491.375806	38.484045
2327.075517	262951.563867	38.489063
2329.499577	263406.223532	38.494080
2331.894987	263845.519471	38.499098
2334.266395	264300.595045	38.504116
2336.865040	264741.383985	38.509133
2339.407224	265183.909769	38.514151
2341.340096	265636.871693	38.519168
2344.135554	266090.865880	38.524186
2346.441938	266530.254985	38.529204
2348.552174	266978.261866	38.534221
2350.776660	267432.296995	38.539239
2352.960954	267882.172730	38.544256
2355.760885	268330.427019	38.549274
2357.663742	268794.218235	38.554292
2360.530705	269233.749185	38.559309
2362.915322	269684.712151	38.564327
2365.196114	270138.384586	38.569344
2368.276903	270569.194433	38.574362
2370.943525	270966.969532	38.579380
2374.065365	271359.591945	38.584397
2377.092250	271740.264546	38.589415
2379.541160	272112.467929	38.594432
2382.015765	272488.401631	38.599450
2384.295244	272870.082110	38.604468
2386.509107	273236.632627	38.609485
2388.792513	273621.259403	38.614503
2390.434453	274020.848898	38.619520
2392.436493	274409.127630	38.624538
2394.597605	274810.108275	38.629556
2397.246122	275197.344626	38.634573
2399.481580	275608.576452	38.639591
2401.348701	276028.630805	38.644608
2403.622224	276445.572280	38.649626
2405.725161	276871.736755	38.654644
2407.643886	277298.946471	38.659661
2409.968965	277736.303831	38.664679
2411.908186	278174.535120	38.669696
2414.705482	278638.236845	38.674714
2416.942282	279084.270257	38.679732
2418.950320	279545.581726	38.684749
2421.385141	280015.589454	38.689767
2423.617680	280480.802330	38.694784
2426.880771	280938.332194	38.699802
2429.585376	281392.012751	38.704820
2432.108843	281842.063616	38.709837
2435.341855	282310.419027	38.714855
2437.109693	282767.117541	38.719872
2439.617055	283224.892393	38.724890
2442.281790	283688.662423	38.729908
2444.908222	284144.766306	38.734925
2447.452830	284614.651170	38.739943
2449.839929	285077.015750	38.744960
2452.410008	285535.413318	38.749978
2454.751051	286001.289719	38.754996
2456.971765	286468.454743	38.760013
2459.579154	286935.100611	38.765031
2462.213575	287410.378540	38.770048
2465.118159	287873.089337	38.775066
2467.509825	288338.471823	38.780084
2469.899645	288797.325364	38.785101
2472.499462	289265.213690	38.790119
2474.612266	289741.586720	38.795136
2477.054165	290201.344222	38.800154
2479.206399	290676.388408	38.805172
2481.492781	291158.828012	38.810189
2484.351708	291641.277563	38.815207
2486.349475	292121.169957	38.820224
2488.808013	292616.255215	38.825242
2491.048254	293101.822705	38.830260
2493.556206	293601.165574	38.835277
2496.110734	294094.581188	38.840295
2498.412087	294589.940935	38.845312
2501.049154	295078.184501	38.850330
2503.782937	295540.958681	38.855348
2505.785289	296010.655415	38.860365
2508.456409	296472.624446	38.865383
2510.654101	296944.243873	38.870400
2513.273891	297402.027422	38.875418
2515.674491	297879.175279	38.880436
2517.815416	298364.288322	38.885453
2520.376753	298833.762201	38.890471
2522.725997	299329.381175	38.895488
2525.579614	299815.723424	38.900506
2528.029691	300299.791237	38.905524
2530.333316	300793.914309	38.910541
2533.640537	301268.521070	38.915559
2536.138774	301752.602177	38.920576
2538.785960	302240.569902	38.925594
2541.275642	302733.387168	38.930612
2543.911013	303230.650247	38.935629
2546.604895	303710.832989	38.940647
2548.860831	304224.460034	38.945664
2551.187209	304722.351030	38.950682
2553.840748	305226.284501	38.955700
2556.139219	305731.491557	38.960717
2558.839740	306244.049876	38.965735
2561.586149	306765.565184	38.970752
2563.947803	307269.968832	38.975770
2566.547102	307790.665023	38.980788
2569.467487	308319.156726	38.985805
2571.839073	308825.686050	38.990823
2574.175260	309352.056009	38.995840
2577.267528	309868.144002	39.000858
2579.729465	310386.666321	39.005876
2581.894339	310930.734308	39.010893
2585.111262	311453.323049	39.015911
2587.408794	311987.230602	39.020928
2590.081229	312505.785973	39.025946
2592.820178	313042.209122	39.030964
2595.562814	313575.022370	39.035981
2598.430073	314100.396786	39.040999
2601.059791	314640.765877	39.046016
2603.815260	315156.932975	39.051034
2606.474415	315674.839776	39.056052
2608.880808	316208.810118	39.061069
2611.876743	316737.325209	39.066087
2614.225179	317262.663688	39.071104
2616.827576	317807.947020	39.076122
2619.491600	318338.994850	39.081140
2622.000776	318873.238872	39.086157
2624.717921	319405.542075	39.091175
2627.310189	319940.173096	39.096192
2630.102034	320464.889938	39.101210
2633.281350	320990.558192	39.106228
2636.060647	321519.435864	39.111245
2638.997126	322026.114320	39.116263
2642.028971	322550.298157	39.121280
2644.566559	323052.259240	39.126298
2647.317032	323529.193940	39.131316
2649.744311	323995.764807	39.136333
2652.235407	324465.497409	39.141351
2654.797265	324947.329810	39.146368
2657.350982	325413.339291	39.151386
2660.290685	325885.786133	39.156404
2662.418805	326388.045643	39.161421
2665.229214	326863.275223	39.166439
2667.150926	327356.444451	39.171456
2669.504093	327850.557994	39.176474
2672.106148	328359.916420	39.181492
2674.482895	328872.430628	39.186509
2677.438456	329380.481884	39.191527
2679.408848	329903.769740	39.196544
2682.047339	330431.061871	39.201562
2684.761989	330954.783045	39.206580
2687.166974	331503.993685	39.211597
2689.622602	332054.385592	39.216615
2691.951423	332601.136737	39.221632
2694.556923	333160.637804	39.226650
2697.343101	333719.547138	39.231668
2699.869823	334286.847153	39.236685
2703.000210	334853.640591	39.241703
2705.486474	335435.969632	39.246720
2708.147058	335995.337272	39.251738
2710.970019	336586.896360	39.256756
2713.490930	337170.982158	39.261773
2716.547497	337757.872488	39.266791
2719.395512	338355.099212	39.271808
2721.820842	338935.477174	39.276826
2724.759560	339525.442267	39.281844
2727.564961	340118.469765	39.286861
2730.841389	340701.184908	39.291879
2734.131013	341292.296449	39.296896
2736.917809	341869.263854	39.301914
2740.041412	342436.499171	39.306932
2742.881695	343022.434882	39.311949
2745.980425	343579.863207	39.316967
2749.175364	344153.037280	39.321984
2751.702490	344712.627281	39.327002
2754.201109	345297.909031	39.332020
2757.140075	345865.470683	39.337037
2759.973647	346424.513228	39.342055
2762.557183	347003.874243	39.347072
2765.550330	347580.727304	39.352090
2768.396629	348142.771866	39.357108
2771.326268	348711.804197	39.362125
2774.606654	349253.891182	39.367143
2777.667767	349815.529279	39.372160
2780.231708	350363.608209	39.377178
2783.561312	350921.308317	39.382196
2786.317326	351482.596587	39.387213
2789.409001	352017.222460	39.392231
2792.245643	352567.114056	39.397248
2794.664123	353097.342473	39.402266
2797.559459	353618.174029	39.407284
2799.903547	354128.096428	39.412301
2802.909850	354621.714192	39.417319
2805.434770	355129.846518	39.422336
2808.009867	355641.824036	39.427354
2810.225281	356162.305781	39.432372
2812.510359	356683.481799	39.437389
2815.544113	357207.605075	39.442407
2817.986774	357753.441846	39.447424
2820.422419	358297.420799	39.452442
2822.872594	358850.249506	39.457460
2825.052913	359421.820525	39.462477
2827.305451	360000.911430	39.467495
2830.328196	360586.269267	39.472512
2832.413872	361188.976018	39.477530
2835.188486	361794.814615	39.482548
2838.173943	362402.413939	39.487565
2840.891700	363014.793616	39.492583
2843.514085	363637.915527	39.497600
2845.902758	364266.446214	39.502618
2848.932451	364905.474804	39.507636
2851.314429	365547.464596	39.512653
2853.826249	366210.259503	39.517671
2856.656562	366875.151179	39.522688
2859.730117	367539.283807	39.527706
2863.033778	368190.529578	39.532724
2866.388163	368861.855288	39.537741
2869.818117	369509.965434	39.542759
2873.458940	370151.130400	39.547776
2876.300962	370803.399452	39.552794
2879.938805	371441.830351	39.557812
2883.094669	372089.031140	39.562829
2886.432775	372715.462874	39.567847
2889.690575	373356.208356	39.572864
2892.231250	373987.238155	39.577882
2895.307992	374622.791171	39.582900
2898.164048	375252.711263	39.587917
2901.576723	375876.190553	39.592935
2904.524906	376500.672454	39.597952
2906.947639	377135.477596	39.602970
2909.959113	377755.439210	39.607988
2912.858176	378390.529421	39.613005
2915.776865	379024.287044	39.618023
2918.501435	379650.454355	39.623040
2921.082645	380292.083841	39.628058
2924.417577	380930.589888	39.633076
2926.926444	381578.272406	39.638093
2930.094768	382214.779313	39.643111
2933.781988	382834.933102	39.648128
2936.482847	383463.071100	39.653146
2940.106435	384091.255442	39.658164
2942.972804	384722.288542	39.663181
2945.842713	385348.693829	39.668199
2949.044615	385962.125158	39.673216
2952.253485	386572.044800	39.678234
2955.078858	387159.973519	39.683252
2957.368272	387742.397508	39.688269
2960.247686	388317.819886	39.693287
2963.402272	388894.077174	39.698304
2965.815539	389484.087482	39.703322
2968.852435	390059.608998	39.708340
2971.881301	390649.299549	39.713357
2974.542369	391235.259587	39.718375
2977.738042	391829.088469	39.723392
2980.496903	392427.490474	39.728410
2983.090510	393034.175600	39.733428
2985.963059	393648.616585	39.738445
2989.028055	394262.229953	39.743463
2991.890567	394885.804841	39.748480
2994.285375	395524.809235	39.753498
2997.120912	396156.733074	39.758516
2999.779178	396805.687643	39.763533
3002.142319	397463.982139	39.768551
3004.608579	398126.557774	39.773568
3007.437537	398800.295198	39.778586
3010.568282	399491.947716	39.783604
3013.642338	400175.861422	39.788621
3016.221537	400867.166298	39.793639
3019.529040	401579.561869	39.798656
3022.152733	402299.934539	39.803674
3025.144376	403008.494631	39.808692
3027.939850	403730.582359	39.813709
3031.208916	404470.882065	39.818727
3034.139328	405201.457951	39.823744
3036.785349	405936.345840	39.828762
3040.213303	406677.962217	39.833780
3042.966792	407422.683957	39.838797
3046.293880	408179.565269	39.843815
3049.071928	408926.325007	39.848832
3052.241299	409685.145510	39.853850
3055.162155	410454.935734	39.858868
3058.676869	411216.983226	39.863885
3061.884698	411984.027353	39.868903
3065.233003	412742.944601	39.873920
3068.856324	413496.375265	39.878938
3072.402429	414254.284442	39.883956
3076.367371	414989.654444	39.888973
3079.824945	415735.982917	39.893991
3083.270165	416442.001979	39.899008
3086.692046	417167.164598	39.904026
3090.725994	417868.570050	39.909044
3094.477356	418556.345134	39.914061
3097.749315	419246.586463	39.919079
3100.950170	419937.658235	39.924096
3103.976096	420620.632712	39.929114
3107.203057	421303.888000	39.934132
3110.217007	421983.841130	39.939149
3113.326908	422651.398685	39.944167
3117.008218	423312.870612	39.949184
3119.751251	423975.462995	39.954202
3122.535941	424621.008555	39.959220
3125.613054	425247.416802	39.964237
3128.137273	425881.624320	39.969255
3130.581000	426514.436352	39.974272
3133.063499	427170.455884	39.979290
3135.822592	427818.740368	39.984308
3138.536318	428484.215131	39.989325
3141.536940	429145.271109	39.994343
3144.915174	429821.321202	39.999360
3147.750115	430495.565508	40.004378
3150.932089	431186.428097	40.009396
3154.132995	431865.112546	40.014413
3157.472693	432561.662585	40.019431
3161.000422	433241.803935	40.024448
3164.594443	433936.934149	40.029466
3167.728714	434620.747729	40.034484
3170.708328	435319.786537	40.039501
3173.760028	436011.147223	40.044519
3176.906013	436713.488932	40.049536
3179.588825	437431.026158	40.054554
3182.586417	438143.606125	40.059572
3185.843542	438864.404059	40.064589
3188.838338	439578.943395	40.069607
3192.041237	440314.746845	40.074624
3195.648336	441029.906611	40.079642
3199.259710	441763.323255	40.084660
3202.235418	442495.957539	40.089677
3205.103289	443241.497305	40.094695
3208.096306	443971.451247	40.099712
3211.268974	444729.908060	40.104730
3214.526390	445485.492324	40.109748
3217.431629	446251.131698	40.114765
3220.103939	447013.745784	40.119783
3223.394234	447799.927679	40.124800
3226.121256	448590.778544	40.129818
3229.353497	449378.839968	40.134836
3232.647401	450166.257480	40.139853
3235.858677	450966.820670	40.144871
3239.556243	451765.001537	40.149888
3243.475697	452547.987118	40.154906
3247.076587	453327.858451	40.159924
3250.569621	454101.748458	40.164941
3253.774976	454893.116013	40.169959
3257.064178	455681.760486	40.174976
3259.994139	456475.241064	40.179994
3263.160329	457260.155344	40.185012
3266.647534	458067.557510	40.190029
3269.287449	458865.248602	40.195047
3272.759407	459676.490048	40.200064
3275.793253	460478.360618	40.205082
3278.570223	461293.800394	40.210100
3282.485275	462093.600180	40.215117
3285.659843	462928.543617	40.220135
3289.339658	463726.347111	40.225152
3292.741513	464536.253982	40.230170
3295.864788	465302.422056	40.235188
3298.839437	466063.123473	40.240205
3302.212122	466835.670692	40.245223
3305.612998	467585.830955	40.250240
3308.910207	468357.626071	40.255258
3312.221738	469114.168432	40.260276
3315.216540	469888.483218	40.265293
3317.930775	470669.892867	40.270311
3320.981403	471451.927640	40.275328
3324.336110	472257.093258	40.280346
3327.425770	473047.100605	40.285364
3330.966665	473839.129472	40.290381
3333.757592	474663.855684	40.295399
3336.950905	475476.957943	40.300416
3340.193576	476301.191862	40.305434
3343.049023	477142.994431	40.310452
3346.272986	477988.898802	40.315469
3349.143673	478856.103314	40.320487
3352.505984	479714.700550	40.325504
3355.549477	480590.950124	40.330522
3358.766149	481470.519361	40.335540
3362.118633	482358.315732	40.340557
3365.077766	483272.563884	40.345575
3368.352334	484161.351285	40.350592
3372.166397	485080.179338	40.355610
3375.221219	485993.070523	40.360628
3378.878240	486915.473330	40.365645
3382.110014	487843.203582	40.370663
3385.751407	488759.961567	40.375680
3389.611284	489689.118498	40.380698
3393.098544	490610.710895	40.385716
3397.103999	491518.436183	40.390733
3400.394106	492448.808728	40.395751
3404.060095	493382.812731	40.400768
3407.294834	494307.140428	40.405786
3410.751767	495232.901552	40.410804
3414.255566	496168.910551	40.415821
3417.347408	497116.753115	40.420839
3420.619765	498061.033356	40.425856
3423.937986	499004.449024	40.430874
3427.078018	499960.162932	40.435892
3430.761503	500896.100174	40.440909
3434.450175	501858.441493	40.445927
3438.204445	502806.787117	40.450944
3441.956069	503753.012541	40.455962
3445.914090	504691.280015	40.460980
3449.492392	505623.046047	40.465997
3452.855102	506565.042027	40.471015
3456.572248	507510.564593	40.476032
3460.033742	508440.835148	40.481050
3463.377699	509371.629095	40.486068
3467.447998	510302.509991	40.491085
3470.359903	511247.096317	40.496103
3473.733887	512186.208923	40.501120
3476.823502	513108.133471	40.506125
3480.139280	513989.467624	40.511130
3483.460632	514822.302984	40.516135
3486.553410	515594.545975	40.521140
3489.769229	516302.356442	40.526144
3492.645572	516945.057060	40.531149
3495.396911	517535.415051	40.536154
3498.293843	518059.436955	40.541159
3500.467815	518511.147987	40.546164
3502.837919	518919.634506	40.551168
3504.959433	519268.284420	40.556173
3506.390076	519570.620781	40.561178
3508.179473	519817.581574	40.566183
3509.422232	520032.974496	40.571188
3511.225093	520187.099128	40.576192
3512.347366	520321.055674	40.581197
3513.057231	520402.697392	40.586202
3514.830108	520451.307557	40.591207
3515.428935	520465.976061	40.596212
3516.103342	520463.644897	40.601216
3517.054384	520431.592033	40.606221
3517.822594	520355.531157	40.611226
3518.510689	520269.471855	40.616231
3518.930511	520167.224879	40.621236
3519.717949	520038.931349	40.626240
3520.102887	519893.611009	40.631245
3519.956032	519729.918695	40.636250
3520.785206	519549.789694	40.641255
3520.883252	519358.549492	40.646260
3521.106747	519153.584746	40.651264
3521.270131	518960.863274	40.656269
3521.429887	518740.077129	40.661274
3521.520643	518515.557146	40.666279
3521.637162	518267.517122	40.671284
3521.581984	518033.305075	40.676288
3521.677188	517782.732833	40.681293
3521.779807	517536.757284	40.686298
3521.635532	517285.254576	40.691303
3521.270525	517024.680477	40.696308
3521.483664	516767.651954	40.701312
3521.591209	516514.530095	40.706317
3521.304994	516251.402875	40.711322
3521.249956	515981.205396	40.716327
3520.908445	515718.280784	40.721332
3520.718049	515451.181076	40.726336
3520.605497	515183.913071	40.731341
3520.333394	514936.137617	40.736346
3520.275648	514665.615836	40.741351
3520.125987	514409.619868	40.746356
3519.567888	514159.855053	40.751360
3519.481593	513901.565317	40.756365
3519.341040	513656.784902	40.761370
3519.459481	513392.537203	40.766375
3518.867653	513150.198019	40.771380
3519.029625	512895.343703	40.776384
3518.784147	512643.331976	40.781389
3518.107479	512417.789059	40.786394
3518.162820	512166.835518	40.791399
3518.128261	511930.207916	40.796404
3517.489676	511691.294970	40.801408
3517.672420	511467.019960	40.806413
3517.052624	511227.186967	40.811418
3517.323086	511008.355408	40.816423
3516.904679	510780.928777	40.821428
3516.639060	510566.729194	40.826432
3516.363019	510341.095387	40.831437
3516.297973	510137.684829	40.836442
3516.102785	509925.995574	40.841447
3516.099414	509712.401509	40.846452
3515.867430	509514.676141	40.851456
3515.721304	509299.885295	40.856461
3515.411511	509096.905799	40.861466
3515.224008	508884.342384	40.866471
3515.045524	508690.090021	40.871476
3514.843306	508498.874901	40.876480
3514.879886	508298.512756	40.881485
3514.095615	508115.126454	40.886490
3513.830213	507934.489591	40.891495
3513.616587	507755.815934	40.896500
3513.750386	507582.904225	40.901504
3513.367911	507412.501085	40.906509
3513.252449	507241.801073	40.911514
3513.609241	507073.554684	40.916519
3513.092106	506912.174509	40.921524
3512.814998	506755.612481	40.926528
3512.990101	506581.216850	40.931533
3512.837952	506423.367066	40.936538
3512.643699	506258.084113	40.941543
3512.567095	506111.453042	40.946548
3512.088069	505962.303629	40.951552
3512.067244	505805.237114	40.956557
3511.811070	505652.102817	40.961562
3511.972419	505499.812048	40.966567
3511.648309	505370.469646	40.971572
3511.555417	505231.424326	40.976576
3511.437477	505093.292742	40.981581
3511.164960	504953.210900	40.986586
3511.196430	504822.644325	40.991591
3510.849228	504686.823012	40.996596
3510.895165	504565.361284	41.001600
3511.005913	504430.224695	41.006605
3510.538098	504310.006348	41.011610
3510.615940	504175.024814	41.016615
3510.454855	504066.497217	41.021620
3510.059181	503941.760864	41.026624
3510.260033	503823.002345	41.031629
3509.813073	503708.545934	41.036634
3509.694253	503590.747328	41.041639
3509.493742	503489.408877	41.046644
3509.362775	503379.252779	41.051648
3509.481016	503259.035833	41.056653
3509.255440	503171.617251	41.061658
3509.463889	503064.138490	41.066663
3509.474213	502977.643262	41.071668
3509.051789	502873.502140	41.076672
3509.420419	502777.839306	41.081677
3509.296389	502660.338976	41.086682
3509.128112	502560.812116	41.091687
3508.509374	502463.835893	41.096692
3508.778800	502362.416694	41.101696
3508.716091	502271.981778	41.106701
3508.360574	502190.247509	41.111706
3508.467157	502098.772689	41.116711
3508.666024	502010.876374	41.121716
3508.400220	501925.533142	41.126720
3508.364154	501841.266697	41.131725
3508.522278	501759.702329	41.136730
3508.258536	501682.000350	41.141735
3508.266230	501572.266610	41.146740
3507.660603	501505.449457	41.151744
3507.995763	501417.123740	41.156749
3507.632592	501347.939372	41.161754
3507.638817	501257.842699	41.166759
3507.542107	501190.437766	41.171764
3507.241316	501127.721513	41.176768
3507.475997	501056.467491	41.181773
3507.526527	500985.343522	41.186778
3507.242878	500919.131288	41.191783
3506.944160	500853.275507	41.196788
3507.318237	500791.767441	41.201792
3507.312415	500709.161212	41.206797
3507.087779	500654.833717	41.211802
3507.172210	500582.994142	41.216807
3506.837651	500529.341667	41.221812
3506.706511	500463.457959	41.226816
3506.930282	500406.831645	41.231821
3506.806726	500350.664996	41.236826
3506.940649	500290.256144	41.241831
3506.654283	500235.127233	41.246836
3506.758119	500175.988215	41.251840
3506.715735	500118.390680	41.256845
3506.146608	500063.710882	41.261850
3506.371007	500008.348685	41.266855
3506.192297	499968.640795	41.271860
3506.278105	499909.908702	41.276864
3506.436980	499858.859056	41.281869
3506.164360	499813.293783	41.286874
3506.221881	499762.917941	41.291879
3506.174007	499728.200210	41.296884
3506.056295	499669.195775	41.301888
3506.194132	499615.516511	41.306893
3505.607798	499574.252322	41.311898
3506.179975	499528.502179	41.316903
3506.023551	499493.649289	41.321908
3505.674834	499442.779928	41.326912
3505.915952	499398.802888	41.331917
3505.859209	499358.213811	41.336922
3505.913313	499311.431336	41.341927
3505.741902	499271.113291	41.346932
3505.786598	499234.152634	41.351936
3505.764974	499190.368477	41.356941
3505.408022	499153.876109	41.361946
3505.618876	499107.321436	41.366951
3505.922604	499068.193381	41.371956
3505.364460	499039.933326	41.376960
3505.563125	499010.895521	41.381965
3505.600175	498973.176205	41.386970
3505.851740	498929.196365	41.391975
3505.644600	498887.617550	41.396980
3505.769841	498850.491506	41.401984
3505.682142	498811.222270	41.406989
3505.548176	498773.681434	41.411994
3505.513131	498733.138137	41.416999
3505.310509	498703.707657	41.422004
3505.266976	498673.492639	41.427008
3505.336880	498633.793121	41.432013
3505.345997	498592.179442	41.437018
3505.374129	498554.359411	41.442023
3505.393302	498543.725483	41.447028
3504.957384	498513.875956	41.452032
3505.141345	498474.512424	41.457037
3505.030049	498446.940161	41.462042
3505.063826	498421.774864	41.467047
3505.292686	498384.023997	41.472052
3505.149022	498360.860989	41.477056
3505.246308	498330.319395	41.482061
3504.938255	498301.411160	41.487066
3505.301224	498268.751883	41.492071
3505.234602	498248.512753	41.497076
3505.192580	498209.994349	41.502080
3505.500345	498172.028070	41.507085
3505.059692	498154.733544	41.512090
3504.847300	498118.266850	41.517095
3504.995579	498095.614228	41.522100
3504.969170	498058.763646	41.527104
3504.862179	498031.949439	41.532109
3504.519758	498021.878603	41.537114
3504.950259	498002.117497	41.542119
3504.917265	497967.647139	41.547124
3504.808136	497945.338763	41.552128
3505.025222	497917.511287	41.557133
3504.974330	497896.864276	41.562138
3504.779426	497871.886232	41.567143
3504.858291	497835.069180	41.572148
3504.732081	497820.914030	41.577152
3504.956235	497783.010774	41.582157
3504.715871	497776.264953	41.587162
3505.063752	497742.088344	41.592167
3504.843552	497724.100427	41.597172
3504.562847	497695.541278	41.602176
3505.260125	497675.484521	41.607181
3505.121577	497652.167917	41.612186
3504.823046	497626.244021	41.617191
3505.156863	497593.436255	41.622196
3504.655233	497569.771923	41.627200
3504.689889	497544.858396	41.632205
3504.713040	497529.464382	41.637210
3504.759403	497495.993106	41.642215
3504.346710	497477.174720	41.647220
3504.196221	497457.707355	41.652224
3504.801510	497429.514013	41.657229
3504.374637	497420.468719	41.662234
3504.681429	497408.978639	41.667239
3504.493320	497377.822399	41.672244
3504.722979	497363.863776	41.677248
3504.566329	497338.220802	41.682253
3504.355150	497331.571454	41.687258
3504.667898	497305.044213	41.692263
3504.475329	497288.874061	41.697268
3504.174531	497277.783693	41.702272
3504.654505	497248.901101	41.707277
3504.391318	497245.398815	41.712282
3504.488572	497214.905969	41.717287
3504.547143	497203.454992	41.722292
3504.344369	497185.970056	41.727296
3504.580029	497172.415356	41.732301
3504.458499	497148.639768	41.737306
3504.498780	497123.117244	41.742311
3504.319227	497117.931012	41.747316
3504.006560	497098.235757	41.752320
3504.247068	497089.996106	41.757325
3504.249895	497083.869745	41.762330
3504.409523	497061.112780	41.767335
3504.282974	497052.222342	41.772340
3504.343984	497034.543685	41.777344
3504.469763	497010.526317	41.782349
3504.384528	497009.628497	41.787354
3504.360429	496981.938960	41.792359
3504.633866	496968.124998	41.797364
3504.415766	496956.768223	41.802368
3504.639087	496930.254569	41.807373
3504.714356	496916.927540	41.812378
3504.553320	496893.816025	41.817383
3504.501559	496870.687209	41.822388
3504.405229	496852.729475	41.827392
3504.356762	496831.574584	41.832397
3504.208900	496818.890289	41.837402
3504.127842	496814.194684	41.842407
3504.235789	496801.368688	41.847412
3504.378093	496781.753062	41.852416
3504.370597	496768.793404	41.857421
3504.569332	496753.573493	41.862426
3504.373109	496724.898202	41.867431
3504.271707	496709.877578	41.872436
3504.158180	496704.680792	41.877440
3504.401844	496683.428927	41.882445
3504.250532	496674.390332	41.887450
3504.433795	496651.274718	41.892455
3504.218930	496637.233912	41.897460
3504.080422	496630.319677	41.902464
3504.402798	496608.194595	41.907469
3504.506645	496608.228816	41.912474
3504.224206	496581.035160	41.917479
3504.129741	496570.063631	41.922484
3504.006268	496560.311775	41.927488
3504.352713	496539.701673	41.932493
3504.216538	496539.065026	41.937498
3504.309541	496521.026409	41.942503
3504.438180	496500.906350	41.947508
3504.285813	496485.235417	41.952512
3504.511325	496463.631761	41.957517
3504.506780	496456.645656	41.962522
3504.701912	496430.743280	41.967527
3504.356787	496424.772951	41.972532
3504.197109	496416.697507	41.977536
3504.601154	496391.116459	41.982541
3504.272579	496390.459587	41.987546
3504.318668	496358.353249	41.992551
3504.502553	496350.122214	41.997556
3504.009013	496331.619192	42.002560
3504.255803	496311.328360	42.007565
3504.291273	496295.627575	42.012570
3504.509475	496291.745239	42.017575
3504.089129	496268.066357	42.022580
3504.198096	496255.594223	42.027584
3504.432703	496241.735218	42.032589
3504.177164	496237.725229	42.037594
3504.206291	496225.620103	42.042599
3504.404188	496196.476646	42.047604
3504.210486	496188.355848	42.052608
3504.371489	496181.242212	42.057613
3504.256621	496160.350185	42.062618
3504.431880	496142.399452	42.067623
3504.253378	496121.061767	42.072628
3504.135085	496104.726929	42.077632
3504.285148	496099.943979	42.082637
3503.997672	496078.167796	42.087642
3504.272523	496080.250830	42.092647
3504.358115	496073.756635	42.097652
3504.454124	496044.831561	42.102656
3504.481170	496031.764658	42.107661
3504.375029	496014.111428	42.112666
3504.639184	495980.805458	42.117671
3504.635166	495973.970977	42.122676
3504.343871	495957.663351	42.127680
3504.565068	495924.870375	42.132685
3504.392946	495915.075231	42.137690
3504.257103	495903.806057	42.142695
3504.367848	495881.359128	42.147700
3504.299702	495868.813462	42.152704
3504.501504	495852.427804	42.157709
3504.256109	495833.682530	42.162714
3504.304502	495826.890341	42.167719
3504.368871	495804.754433	42.172724
3503.879965	495797.591477	42.177728
3504.322078	495774.788256	42.182733
3503.776903	495779.127442	42.187738
3504.056296	495759.134630	42.192743
3504.217005	495748.983004	42.197748
3504.234969	495751.258573	42.202752
3504.077747	495731.233478	42.207757
3503.904070	495716.831032	42.212762
3504.214788	495707.617666	42.217767
3504.247177	495702.600055	42.222772
3504.089276	495678.220717	42.227776
3504.371187	495671.189035	42.232781
3504.383097	495653.516797	42.237786
3504.311274	495641.477870	42.242791
3504.209021	495632.177846	42.247796
3504.281489	495614.546630	42.252800
3504.553669	495590.605513	42.257805
3504.243565	495585.388845	42.262810
3504.305593	495557.936687	42.267815
3504.352490	495556.258434	42.272820
3503.900916	495540.330189	42.277824
3504.451286	495522.218295	42.282829
3504.168009	495516.237890	42.287834
3504.053660	495491.395732	42.292839
3504.548310	495471.925533	42.297844
3504.245829	495469.087328	42.302848
3504.379449	495450.281753	42.307853
3504.095863	495441.921668	42.312858
3504.064549	495431.496425	42.317863
3504.346656	495397.578970	42.322868
3504.243177	495400.582627	42.327872
3504.365630	495373.373802	42.332877
3504.170225	495365.303538	42.337882
3504.268710	495345.288235	42.342887
3504.313215	495333.939571	42.347892
3504.318506	495317.432597	42.352896
3504.174047	495298.012598	42.357901
3504.204178	495291.982582	42.362906
3504.189702	495268.390146	42.367911
3504.620127	495262.347485	42.372916
3503.984771	495246.954356	42.377920
3504.408365	495230.684984	42.382925
3504.085765	495215.596824	42.387930
3503.914584	495181.902512	42.392935
3504.092512	495186.178178	42.397940
3503.927462	495182.761245	42.402944
3503.895588	495168.437219	42.407949
3503.805471	495158.476808	42.412954
3503.853863	495152.950189	42.417959
3504.216122	495143.829660	42.422964
3504.051576	495152.311357	42.427968
3504.105598	495121.163613	42.432973
3504.306449	495119.511619	42.437978
3504.307806	495113.081030	42.442983
3504.427143	495089.011516	42.447988
3504.365893	495081.527518	42.452992
3504.694101	495056.260388	42.457997
3504.174883	495051.025985	42.463002
3504.308437	495029.789600	42.468007
3504.041680	495001.629076	42.473012
3504.093909	494995.038505	42.478016
3504.091956	494988.557762	42.483021
3503.966107	494957.083735	42.488026
3504.339658	494953.328463	42.493031
3503.919922	494956.584713	42.498036
3503.950754	494938.098659	42.503040
3504.056210	494922.081831	42.508045
3504.013414	494917.025254	42.513050
3503.883257	494914.868593	42.518055
3504.466205	494906.270033	42.523060
3504.034029	494885.325432	42.528064
3504.270467	494881.034848	42.533069
3504.592541	494859.363400	42.538074
3504.121035	494841.665517	42.543079
3504.028042	494827.198983	42.548084
3503.892194	494821.954553	42.553088
3504.095457	494801.770194	42.558093
3503.696166	494813.934783	42.563098
3504.268207	494807.616420	42.568103
3504.369214	494771.751714	42.573108
3503.828595	494772.039704	42.578112
3504.064830	494759.191997	42.583117
3504.144269	494737.963827	42.588122
3504.206828	494732.181672	42.593127
3504.059570	494722.381957	42.598132
3503.766750	494708.706424	42.603136
3503.940679	494688.020236	42.608141
3503.905696	494677.139435	42.613146
3503.925475	494688.377089	42.618151
3504.178626	494673.956992	42.623156
3503.866332	494658.765474	42.628160
3503.973277	494649.988860	42.633165
3504.029753	494654.688921	42.638170
3503.911262	494638.656607	42.643175
3504.307600	494612.719854	42.648180
3503.856457	494614.816538	42.653184
3504.111128	494598.725209	42.658189
3503.976609	494596.214759	42.663194
3503.846818	494577.044847	42.668199
3504.302254	494570.137222	42.673204
3503.911736	494567.110251	42.678208
3504.145069	494539.983932	42.683213
3504.150346	494536.793129	42.688218
3504.131702	494519.833509	42.693223
3504.317240	494507.196178	42.698228
3504.101938	494507.432752	42.703232
3504.397577	494489.410737	42.708237
3503.833722	494469.195357	42.713242
3503.843778	494452.433677	42.718247
3503.972568	494439.045746	42.723252
3503.790489	494448.138157	42.728256
3503.861063	494445.088922	42.733261
3503.512924	494421.851942	42.738266
3503.892072	494416.576631	42.743271
3503.808517	494412.184611	42.748276
3504.106139	494407.934881	42.753280
3504.065040	494405.055195	42.758285
3503.868172	494388.123622	42.763290
3503.482718	494367.930568	42.768295
3504.104026	494372.743965	42.773300
3503.682619	494364.607709	42.778304
3503.799309	494364.488001	42.783309
3504.032243	494353.159582	42.788314
3504.112568	494335.019543	42.793319
3503.881436	494326.954467	42.798324
3503.873711	494338.399223	42.803329
3503.807871	494314.763042	42.808333
3503.682109	494298.984757	42.813338
3503.929167	494294.742993	42.818343
3504.079088	494296.187724	42.823348
3503.955092	494295.143989	42.828353
3503.848172	494253.032369	42.833357
3503.864816	494255.409603	42.838362
3503.648605	494265.570840	42.843367
3503.549110	494248.927560	42.848372
3503.573102	494262.645939	42.853377
3503.975141	494254.025036	42.858381
3504.087751	494232.234050	42.863386
3503.841550	494227.057527	42.868391
3503.809770	494219.872331	42.873396
3503.965867	494225.569463	42.878401
3504.061353	494212.946163	42.883405
3503.881827	494196.011672	42.888410
3504.058048	494194.009042	42.893415
3504.238874	494187.245949	42.898420
3503.925895	494168.661555	42.903425
3504.057494	494156.083143	42.908429
3503.956347	494153.972442	42.913434
3503.873526	494138.339138	42.918439
3503.968041	494115.791340	42.923444
3503.530489	494114.392069	42.928449
3503.713772	494108.337458	42.933453
3504.063068	494109.041790	42.938458
3503.725847	494105.348054	42.943463
3503.841616	494085.733731	42.948468
3503.780960	494077.033970	42.953473
3503.886591	494058.535208	42.958477
3504.319656	494070.011733	42.963482
3504.075194	494063.467721	42.968487
3503.914991	494043.846337	42.973492
3504.047960	494030.457449	42.978497
3504.231904	494028.149764	42.983501
3503.948837	494012.041644	42.988506
3504.094326	494000.574922	42.993511
3503.867373	493987.445435	42.998516
3503.584444	494000.250436	43.003521
3503.750157	493980.931923	43.008525
3503.736452	493961.236660	43.013530
3503.587049	493953.107865	43.018535
3503.813197	493954.591210	43.023540
3503.734758	493953.844072	43.028545
3503.802716	493953.175067	43.033549
3503.947646	493951.734354	43.038554
3503.996606	493933.953329	43.043559
3504.269972	493916.440636	43.048564
3503.604062	493924.242599	43.053569
3503.763558	493911.811520	43.058573
3503.833086	493904.964642	43.063578
3503.441276	493909.280022	43.068583
3503.713254	493891.970070	43.073588
3503.712156	493896.223698	43.078593
3503.795583	493890.792434	43.083597
3503.797794	493896.362083	43.088602
3503.631141	493897.907518	43.093607
3504.007670	493862.098760	43.098612
3503.546441	493860.804484	43.103617
3503.912535	493858.214807	43.108621
3503.899376	493859.533439	43.113626
3503.851215	493853.110235	43.118631
3504.092362	493826.487993	43.123636
3503.586797	493826.213452	43.128641
3503.606356	493818.159164	43.133645
3503.894701	493814.670313	43.138650
3503.821109	493821.771060	43.143655
3504.159279	493801.665554	43.148660
3503.904361	493789.755623	43.153665
3504.092574	493778.130100	43.158669
3503.944332	493774.254517	43.163674
3504.100788	493768.963584	43.168679
3504.288390	493754.148034	43.173684
3503.866215	493747.176268	43.178689
3504.001766	493726.393792	43.183693
3503.790307	493710.679183	43.188698
3503.886487	493700.485987	43.193703
3504.042408	493699.803070	43.198708
3504.050945	493704.966682	43.203713
3504.201347	493678.459844	43.208717
3503.877555	493662.965497	43.213722
3503.752640	493661.415501	43.218727
3503.680785	493653.223679	43.223732
3503.242810	493666.711699	43.228737
3503.814813	493652.848049	43.233741
3503.967237	493630.239866	43.238746
3503.664734	493629.021759	43.243751
3504.028087	493628.052868	43.248756
3503.692831	493632.460647	43.253761
3503.957491	493632.570733	43.258765
3504.082929	493611.283355	43.263770
3503.927901	493598.699229	43.268775
3503.827012	493588.283935	43.273780
3503.534054	493588.431519	43.278785
3504.022509	493588.151772	43.283789
3503.868765	493556.527842	43.288794
3503.617952	493549.478279	43.293799
3504.127862	493554.360139	43.298804
3503.781257	493553.807281	43.303809
3503.914526	493533.632595	43.308813
3503.798150	493518.510441	43.313818
3503.965655	493519.901816	43.318823
3504.060347	493508.797278	43.323828
3503.920440	493519.200052	43.328833
3504.061889	493481.250306	43.333837
3504.049297	493471.580551	43.338842
3503.594623	493481.881185	43.343847
3503.626910	493466.887403	43.348852
3503.769441	493459.269259	43.353857
3503.966244	493442.223955	43.358861
3503.944368	493443.138894	43.363866
3504.112799	493436.478760	43.368871
3504.094858	493420.986505	43.373876
3503.730258	493415.727190	43.378881
3503.877527	493398.082023	43.383885
3503.803750	493390.903141	43.388890
3503.514963	493398.341891	43.393895
3503.886706	493394.789142	43.398900
3503.943681	493382.272635	43.403905
3503.620884	493362.423035	43.408909
3503.806616	493368.166387	43.413914
3503.587245	493360.959868	43.418919
3503.890112	493346.227048	43.423924
3503.912483	493373.162807	43.428929
3503.944802	493340.395068	43.433933
3503.894200	493331.338901	43.438938
3503.688201	493331.725931	43.443943
3503.991011	493318.664147	43.448948
3503.703534	493313.038147	43.453953
3503.810662	493293.221796	43.458957
3503.625764	493282.211951	43.463962
3503.587315	493280.698894	43.468967
3503.599687	493273.405075	43.473972
3503.671423	493277.140953	43.478977
3503.631045	493282.666881	43.483981
3503.880626	493272.702394	43.488986
3503.831861	493249.467250	43.493991
3504.018770	493241.082432	43.498996
3504.172292	493238.019887	43.504001
3503.958311	493231.825227	43.509005
3503.716438	493199.201851	43.514010
3503.814960	493204.452657	43.519015
3503.809053	493189.717878	43.524020
3503.801402	493191.238240	43.529025
3503.671648	493187.207697	43.534029
3504.022579	493170.239057	43.539034
3503.641398	493153.386118	43.544039
3503.567187	493150.663383	43.549044
3503.696849	493156.213111	43.554049
3503.711118	493146.994685	43.559053
3503.682824	493158.899170	43.564058
3503.643230	493153.740326	43.569063
3503.882346	493130.510169	43.574068
3503.557362	493118.408324	43.579073
3503.724322	493120.306200	43.584077
3503.896840	493120.430854	43.589082
3503.744060	493112.352859	43.594087
3503.947092	493114.042481	43.599092
3503.877869	493095.215920	43.604097
3503.636810	493083.202064	43.609101
3503.582682	493078.855712	43.614106
3503.564316	493076.984995	43.619111
3503.836078	493070.764144	43.624116
3503.667270	493076.209156	43.629121
3504.020074	493065.266109	43.634125
3503.721298	493052.704331	43.639130
3503.453412	493051.581990	43.644135
3503.648302	493047.246910	43.649140
3503.816834	493044.232599	43.654145
3503.769434	493047.734162	43.659149
3503.681258	493043.697015	43.664154
3503.362375	493028.049441	43.669159
3503.688734	493006.527055	43.674164
3503.731744	493001.557666	43.679169
3503.649227	493001.925186	43.684173
3503.858267	493000.524905	43.689178
3503.991246	492998.832814	43.694183
3503.885578	493000.723155	43.699188
3503.894388	492979.200289	43.704193
3503.731195	492966.009356	43.709197
3503.673374	492969.158109	43.714202
3503.683608	492975.233156	43.719207
3503.899249	492959.399761	43.724212
3503.840448	492945.989758	43.729217
3503.950602	492937.414378	43.734221
3503.844441	492931.506409	43.739226
3503.661960	492923.483665	43.744231
3503.914617	492925.317378	43.749236
3503.489085	492916.472184	43.754241
3503.795562	492898.801377	43.759245
3503.872738	492890.180548	43.764250
3503.402578	492893.242570	43.769255
3503.713402	492887.977626	43.774260
3503.865872	492902.335019	43.779265
3503.619723	492892.651237	43.784269
3503.762087	492884.020102	43.789274
3503.757709	492865.385614	43.794279
3504.061689	492858.146818	43.799284
3503.762714	492857.282574	43.804289
3503.633369	492850.416100	43.809293
3503.767761	492858.294571	43.814298
3503.722634	492846.958540	43.819303
3503.753298	492813.531818	43.824308
3503.694751	492825.694496	43.829313
3503.425712	492816.824520	43.834317
3503.707620	492822.451563	43.839322
3503.573202	492812.193047	43.844327
3503.715550	492818.145986	43.849332
3503.571456	492830.777935	43.854337
3503.609124	492800.033960	43.859341
3503.473285	492790.028853	43.864346
3503.432538	492787.250136	43.869351
3503.769161	492779.297199	43.874356
3503.756897	492787.806553	43.879361
3503.725511	492792.369058	43.884365
3504.003439	492772.373234	43.889370
3503.407961	492782.038199	43.894375
3503.657189	492756.780401	43.899380
3503.734757	492752.311878	43.904385
3503.682568	492746.294040	43.909389
3503.677666	492745.231392	43.914394
3503.592241	492747.473036	43.919399
3503.464409	492739.897329	43.924404
3503.448100	492750.736754	43.929409
3503.622673	492748.379753	43.934413
3503.589723	492748.030491	43.939418
3503.237838	492741.553626	43.944423
3503.446976	492719.745597	43.949428
3503.271766	492717.798355	43.954433
3503.589585	492718.710278	43.959437
3503.513579	492724.090086	43.964442
3503.654680	492715.155235	43.969447
3503.679923	492711.150728	43.974452
3503.658499	492714.546969	43.979457
3503.639565	492719.867117	43.984461
3503.863355	492715.426113	43.989466
3503.692934	492716.668404	43.994471
3503.593951	492699.567887	43.999476
3503.693491	492693.779248	44.004481
3503.694180	492687.094719	44.009485
3503.848796	492693.450875	44.014490
3503.386100	492690.586918	44.019495
3503.781811	492691.233333	44.024500
3503.822950	492692.897943	44.029505
3503.775298	492670.826607	44.034509
3503.766626	492665.662738	44.039514
3503.642145	492652.060345	44.044519
3503.624782	492648.670235	44.049524
3503.439260	492659.181981	44.054529
3503.438862	492657.308381	44.059533
3503.821334	492647.626392	44.064538
3503.466023	492654.569557	44.069543
3503.816953	492633.802449	44.074548
3503.472188	492629.198090	44.079553
3503.453086	492627.175525	44.084557
3503.648929	492619.497969	44.089562
3503.896187	492620.015932	44.094567
3504.035793	492621.259867	44.099572
3503.723422	492627.082180	44.104577
3503.973035	492600.608754	44.109581
3504.232100	492574.690836	44.114586
3503.782534	492587.067394	44.119591
3503.999747	492594.173289	44.124596
3503.944699	492571.596605	44.129601
3504.034928	492548.895651	44.134605
3504.117395	492552.832541	44.139610
3503.927241	492540.607724	44.144615
3503.970869	492517.610258	44.149620
3503.626370	492506.270696	44.154625
3503.796305	492504.927199	44.159629
3504.032390	492508.130857	44.164634
3503.632323	492503.433927	44.169639
3503.783553	492480.419407	44.174644
3503.837904	492472.510954	44.179649
3503.890559	492459.893225	44.184653
3503.766104	492461.128267	44.189658
3503.953566	492484.190571	44.194663
3503.976509	492451.068256	44.199668
3503.948414	492436.083183	44.204673
3503.917310	492420.592169	44.209677
3503.768176	492424.717614	44.214682
3503.808846	492414.431203	44.219687
3503.824996	492402.680091	44.224692
3503.673344	492382.447903	44.229697
3503.716473	492394.392231	44.234701
3503.792153	492393.418108	44.239706
3503.813176	492387.894986	44.244711
3503.896318	492378.462729	44.249716
3503.740530	492350.888294	44.254721
3503.851787	492344.439367	44.259725
3503.909030	492344.177122	44.264730
3503.667898	492354.748471	44.269735
3503.597648	492330.198915	44.274740
3503.773207	492315.586680	44.279745
3503.739395	492299.133821	44.284749
3503.650460	492306.693341	44.289754
3503.655554	492318.339886	44.294759
3503.822104	492309.147615	44.299764
3503.834176	492312.437354	44.304769
3503.582103	492306.349685	44.309773
3503.754242	492277.609214	44.314778
3503.298893	492274.693389	44.319783
3503.558870	492270.499763	44.324788
3503.568543	492266.345698	44.329793
3503.582019	492267.508312	44.334797
3503.846977	492264.630556	44.339802
3503.769340	492263.933863	44.344807
3503.968869	492259.851070	44.349812
3504.194655	492234.343063	44.354817
3503.869572	492237.584823	44.359821
3504.195306	492233.785923	44.364826
3503.861339	492228.015017	44.369831
3503.865820	492201.022717	44.374836
3504.030314	492199.376213	44.379841
3503.714274	492188.285162	44.384845
3503.670610	492190.874758	44.389850
3503.611351	492188.605287	44.394855
3503.586481	492155.439361	44.399860
3503.747282	492154.958182	44.404865
3503.756771	492154.247713	44.409869
3503.637840	492142.365864	44.414874
3503.667371	492151.172750	44.419879
3503.801594	492140.314349	44.424884
3503.824730	492129.372217	44.429889
3503.834771	492124.661011	44.434893
3503.837164	492120.457423	44.439898
3503.613508	492127.025487	44.444903
3503.833194	492115.191382	44.449908
3504.106919	492110.742341	44.454913
3504.138462	492086.429580	44.459917
3503.835702	492079.590228	44.464922
3503.646745	492089.292579	44.469927
3503.873017	492086.471553	44.474932
3503.786595	492065.215883	44.479937
3503.600212	492049.495896	44.484941
3503.772444	492043.087869	44.489946
3503.312859	492045.641942	44.494951
3503.716966	492032.613884	44.499956
3503.918092	492043.520638	44.504961
3503.677427	492039.456732	44.509965
3503.881651	492016.230695	44.514970
3503.712968	492005.977148	44.519975
3503.615516	492002.700861	44.524980
3503.646484	492002.999821	44.529985
3503.580782	492007.010888	44.534989
3503.839781	491998.917963	44.539994
3503.594687	491995.867577	44.544999
3503.868721	491971.009921	44.550004
3503.928295	491961.834386	44.555009
3503.887532	491962.245968	44.560013
3503.709982	491958.779767	44.565018
3503.566348	491961.537122	44.570023
3503.617047	491960.111149	44.575028
3503.658812	491944.051163	44.580033
3503.522030	491930.095692	44.585037
3503.695818	491942.222227	44.590042
3503.404943	491944.597723	44.595047
3503.498557	491932.277012	44.600052
3503.463953	491931.269654	44.605057
3503.562941	491933.279680	44.610061
3503.639766	491925.823217	44.615066
3503.439226	491932.185130	44.620071
3503.758591	491931.071182	44.625076
3503.781084	491923.319456	44.630081
3504.024997	491908.645455	44.635085
3504.145891	491899.308272	44.640090
3503.582530	491900.511440	44.645095
3503.865782	491885.426069	44.650100
3503.704446	491872.588556	44.655105
3503.798729	491864.319039	44.660109
3504.009957	491853.904077	44.665114
3503.602830	491844.397114	44.670119
3503.963965	491854.063283	44.675124
3503.779788	491838.798546	44.680129
3503.741205	491818.497229	44.685133
3503.825968	491804.709215	44.690138
3503.821393	491810.432490	44.695143
3503.961382	491797.800508	44.700148
3503.908517	491798.821710	44.705153
3503.828005	491778.425693	44.710157
3503.953009	491762.858814	44.715162
3503.944940	491771.975676	44.720167
3503.993433	491757.433728	44.725172
3503.987026	491744.723564	44.730177
3503.740102	491733.368105	44.735181
3503.931798	491719.309915	44.740186
3503.684557	491725.527352	44.745191
3503.945696	491728.119479	44.750196
3503.701538	491708.458241	44.755201
3503.464910	491697.962051	44.760205
3504.031720	491685.313173	44.765210
3503.927641	491695.559379	44.770215
3503.987826	491681.977728	44.775220
3503.738361	491671.939334	44.780225
3503.470376	491648.179765	44.785229
3503.752390	491636.234219	44.790234
3503.643172	491650.785872	44.795239
3503.728906	491649.455623	44.800244
3503.878523	491642.493966	44.805249
3503.908095	491638.893683	44.810253
3503.932284	491615.594317	44.815258
3504.013229	491613.606470	44.820263
3503.710386	491615.122976	44.825268
3503.780308	491617.492129	44.830273
3503.679220	491603.581414	44.835277
3503.957207	491575.582767	44.840282
3503.929296	491564.749656	44.845287
3503.721862	491574.910980	44.850292
3503.823566	491570.590285	44.855297
3503.784023	491565.988060	44.860301
3503.798801	491534.789823	44.865306
3503.696235	491543.060806	44.870311
3503.679448	491523.920505	44.875316
3503.582390	491537.457469	44.880321
3503.163389	491548.158673	44.885325
3503.812810	491537.269132	44.890330
3503.557312	491542.069939	44.895335
3503.740584	491530.646360	44.900340
3503.897522	491512.592729	44.905345
3503.523374	491500.598879	44.910349
3503.685452	491498.496911	44.915354
3503.459799	491509.674006	44.920359
3503.682426	491499.712829	44.925364
3503.900850	491497.703240	44.930369
3503.685768	491491.913313	44.935373
3503.823225	491478.369943	44.940378
3503.684964	491473.935226	44.945383
3503.927784	491486.557577	44.950388
3503.862415	491466.006894	44.955393
3503.747831	491475.393952	44.960397
3504.042390	491449.823356	44.965402
3503.671978	491438.183376	44.970407
3503.792862	491429.808177	44.975412
3503.659499	491428.715115	44.980417
3503.585791	491431.562781	44.985421
3503.745170	491428.802872	44.990426
3503.517025	491412.734445	44.995431
3503.351068	491398.985759	45.000436
3503.488408	491397.647336	45.005441
3503.487200	491387.822764	45.010445
3503.502205	491388.883905	45.015450
3503.497228	491396.481168	45.020455
3503.491030	491388.835040	45.025460
3503.829173	491389.338674	45.030465
3503.719470	491395.129337	45.035469
3503.660295	491395.898343	45.040474
3503.526389	491400.376108	45.045479
3503.757248	491383.323531	45.050484
3503.632517	491371.999180	45.055489
3503.576986	491352.054535	45.060493
3503.744956	491347.672672	45.065498
3503.539234	491351.756654	45.070503
3503.914434	491346.126599	45.075508
3503.803811	491350.144906	45.080513
3503.407391	491339.926987	45.085517
3503.603032	491314.827630	45.090522
3503.441638	491322.652220	45.095527
3503.474703	491308.061716	45.100532
3503.622925	491314.925790	45.105537
3503.376053	491318.054060	45.110541
3503.679153	491310.561587	45.115546
3503.525281	491319.651072	45.120551
3503.560009	491317.417282	45.125556
3503.441907	491316.625661	45.130561
3503.364931	491319.676434	45.135565
3503.288122	491325.006130	45.140570
3503.349828	491318.615323	45.145575
3503.363288	491330.565025	45.150580
3503.324555	491322.518866	45.155585
3503.394535	491328.281149	45.160589
3503.644507	491321.202224	45.165594
3503.443275	491347.923051	45.170599
3503.675930	491324.033295	45.175604
3503.899067	491308.551813	45.180609
3503.543305	491290.224499	45.185613
3503.936932	491279.780387	45.190618
3503.573692	491288.295258	45.195623
3503.978217	491281.597037	45.200628
3503.736425	491279.558879	45.205633
3503.765336	491255.751882	45.210637
3503.681365	491243.762645	45.215642
3503.548161	491250.975086	45.220647
3503.965097	491246.047413	45.225652
3503.614776	491245.748285	45.230657
3503.653166	491247.464104	45.235661
3503.635167	491222.246459	45.240666
3503.579360	491211.265622	45.245671
3503.305025	491208.523589	45.250676
3503.583061	491208.935441	45.255681
3503.481623	491208.850193	45.260685
3503.901459	491201.744374	45.265690
3503.748481	491210.428622	45.270695
3503.653930	491198.643603	45.275700
3503.632154	491210.801526	45.280705
3503.390296	491192.405469	45.285709
3503.652846	491177.981166	45.290714
3503.551817	491172.527618	45.295719
3503.832210	491168.735669	45.300724
3503.635590	491170.741858	45.305729
3503.884318	491172.829587	45.310733
3503.947311	491160.057412	45.315738
3503.759717	491159.783206	45.320743
3503.865808	491136.470295	45.325748
3503.870759	491125.226584	45.330753
3503.736134	491118.765453	45.335757
3503.803916	491128.174505	45.340762
3503.762877	491129.953532	45.345767
3503.725665	491105.042629	45.350772
3504.054874	491097.242080	45.355777
3503.646611	491088.190704	45.360781
3503.914703	491086.578373	45.365786
3503.933460	491083.536776	45.370791
3504.099165	491063.911362	45.375796
3504.088288	491049.428890	45.380801
3503.679933	491050.962117	45.385805
3503.824937	491043.393237	45.390810
3503.499856	491036.506384	45.395815
3503.585305	491014.715907	45.400820
3503.784398	491013.823494	45.405825
3503.515988	491010.016967	45.410829
3503.763186	491010.940141	45.415834
3503.152125	491000.857248	45.420839
3503.572562	491011.831233	45.425844
3503.705682	491005.175811	45.430849
3503.435283	491011.346501	45.435853
3504.048985	491005.830579	45.440858
3503.266982	490998.357557	45.445863
3503.728838	490971.898913	45.450868
3503.903051	490977.999340	45.455873
3503.510342	490976.086290	45.460877
3503.612999	490965.890570	45.465882
3503.719091	490967.899579	45.470887
3503.638204	490973.078086	45.475892
3503.732170	490965.922396	45.480897
3503.514422	490951.827055	45.485901
3503.521137	490938.861046	45.490906
3503.576658	490934.243638	45.495911
3503.732903	490928.951932	45.500916
3503.959174	490931.195171	45.505921
3503.581575	490935.508988	45.510925
3503.744004	490930.975971	45.515930
3503.710244	490927.740071	45.520935
3503.664215	490901.310958	45.525940
3503.904919	490899.095206	45.530945
3503.764628	490899.319964	45.535949
3503.781246	490899.519921	45.540954
3503.817613	490898.602579	45.545959
3504.055626	490887.169954	45.550964
3504.066059	490863.821178	45.555969
3503.613570	490866.070420	45.560973
3503.787649	490859.712339	45.565978
3503.697528	490869.703570	45.570983
3503.649259	490850.466264	45.575988
3503.825327	490827.800287	45.580993
3503.679394	490821.695353	45.585997
3503.938852	490813.855066	45.591002
3503.716442	490828.982342	45.596007
3503.966046	490809.799203	45.601012
3503.853927	490786.013897	45.606017
3503.573977	490780.385935	45.611021
3503.720652	490775.348922	45.616026
3503.822013	490776.295158	45.621031
3503.443697	490772.202085	45.626036
3503.826074	490770.571664	45.631041
3503.834694	490762.315199	45.636045
3504.004085	490738.687918	45.641050
3503.501828	490745.756306	45.646055
3504.074094	490739.082024	45.651060
3504.013022	490739.243617	45.656065
3503.687740	490732.660552	45.661069
3503.637809	490707.396614	45.666074
3503.604425	490705.173517	45.671079
3503.743654	490706.670866	45.676084
3503.753218	490708.695160	45.681089
3503.510282	490713.139678	45.686093
3503.792338	490696.382252	45.691098
3503.648829	490687.238188	45.696103
3503.625341	490653.562918	45.701108
3503.745205	490658.760427	45.706113
3503.537964	490660.717704	45.711117
3503.755726	490656.226520	45.716122
3503.744389	490657.950252	45.721127
3503.715978	490658.005393	45.726132
3504.045496	490655.117189	45.731137
3503.790357	490642.597523	45.736141
3503.717477	490614.754184	45.741146
3503.535959	490626.481928	45.746151
3503.532494	490620.708926	45.751156
3504.080231	490613.532024	45.756161
3503.765998	490603.503290	45.761165
3503.833905	490576.954418	45.766170
3503.806254	490585.669793	45.771175
3503.846507	490579.180833	45.776180
3503.819291	490582.173216	45.781185
3503.727514	490568.716064	45.786189
3503.998238	490542.540250	45.791194
3503.884514	490541.444031	45.796199
3503.745669	490544.859227	45.801204
3504.032564	490536.913197	45.806209
3503.537412	490516.125526	45.811213
3503.597020	490496.769514	45.816218
3503.613647	490487.144232	45.821223
3503.767233	490481.447655	45.826228
3503.610186	490490.284817	45.831233
3503.603813	490488.918399	45.836237
3504.022252	490482.977378	45.841242
3503.663759	490481.767907	45.846247
3504.007275	490466.216055	45.851252
3504.069290	490453.342260	45.856257
3504.017804	490461.453711	45.861261
3503.961062	490443.027655	45.866266
3503.601700	490419.078379	45.871271
3503.477313	490407.550804	45.876276
3503.478019	490411.602363	45.881281
3503.620891	490405.046477	45.886285
3503.753610	490405.329381	45.891290
3503.680269	490408.886186	45.896295
3503.865020	490408.198595	45.901300
3503.758894	490385.779269	45.906305
3503.461528	490371.088323	45.911309
3503.237187	490367.933095	45.916314
3503.438954	490373.117739	45.921319
3503.376678	490370.038188	45.926324
3503.573656	490372.032896	45.931329
3503.306777	490383.318472	45.936333
3503.703269	490363.149386	45.941338
3503.905303	490370.461117	45.946343
3503.705742	490362.997069	45.951348
3503.797033	490370.022428	45.956353
3503.482759	490344.546552	45.961357
3503.560127	490330.252158	45.966362
3503.589540	490337.337956	45.971367
3503.415645	490323.589731	45.976372
3503.737615	490321.057191	45.981377
3503.230086	490327.569462	45.986381
3503.257151	490331.566226	45.991386
3502.947207	490335.616255	45.996391
3502.981292	490337.839298	46.001396
3503.336456	490333.123735	46.006401
3503.382643	490329.672512	46.011405
3503.437880	490327.384716	46.016410
3503.509573	490340.997166	46.021415
3503.588269	490325.638992	46.026420
3503.580200	490333.490407	46.031425
3503.728203	490337.518699	46.036429
3503.776396	490338.625300	46.041434
3503.864410	490341.751446	46.046439
3503.465360	490326.975245	46.051444
3503.721817	490306.271126	46.056449
3503.442109	490310.721551	46.061453
3503.897487	490295.658337	46.066458
3503.636976	490299.194101	46.071463
3503.678942	490296.756460	46.076468
3503.720265	490292.445015	46.081473
3503.442847	490297.857357	46.086477
3503.480634	490296.686530	46.091482
3503.689020	490272.849913	46.096487
3503.405042	490260.030672	46.101492
3503.525173	490254.693837	46.106497
3503.619189	490256.958063	46.111501
3503.709928	490250.258425	46.116506
3503.576198	490258.585549	46.121511
3503.431235	490259.874622	46.126516
3503.591106	490261.115514	46.131521
3503.353729	490263.786642	46.136525
3503.754542	490255.113441	46.141530
3503.629511	490249.308893	46.146535
3503.162726	490234.290093	46.151540
3503.653764	490233.250207	46.156545
3503.593294	490229.967763	46.161549
3503.701249	490227.570329	46.166554
3503.523910	490236.765342	46.171559
3503.464903	490234.748824	46.176564
3503.559027	490229.568032	46.181569
3503.237650	490235.747034	46.186573
3503.388144	490227.771787	46.191578
3503.504732	490240.465580	46.196583
3503.326783	490241.405345	46.201588
3503.350472	490246.719463	46.206593
3503.568685	490244.709775	46.211597
3503.712159	490233.443633	46.216602
3503.485194	490245.026861	46.221607
3503.556361	490226.833606	46.226612
3503.714327	490209.436956	46.231617
3503.288300	490203.882554	46.236621
3503.493083	490192.150880	46.241626
3503.728705	490198.900259	46.246631
3503.273109	490202.061704	46.251636
3503.721717	490191.557650	46.256641
3503.447333	490193.323002	46.261645
3503.988633	490205.392580	46.266650
3503.598357	490200.744160	46.271655
3503.305253	490187.825019	46.276660
3503.642601	490169.589637	46.281665
3503.266559	490158.253625	46.286669
3503.525639	490151.932516	46.291674
3503.374693	490163.554425	46.296679
3503.169424	490166.321784	46.301684
3503.514894	490161.101246	46.306689
3503.244247	490159.422050	46.311693
3503.682349	490153.123292	46.316698
3503.423293	490166.484267	46.321703
3503.280888	490161.999246	46.326708
3503.452008	490159.490528	46.331713
3503.275446	490174.155267	46.336717
3503.506588	490167.433408	46.341722
3503.852326	490166.872303	46.346727
3503.873441	490168.489658	46.351732
3503.839581	490161.607096	46.356737
3503.291929	490161.491077	46.361741
3503.599775	490131.611629	46.366746
3503.753629	490130.574386	46.371751
3503.704608	490120.706058	46.376756
3503.747285	490118.774749	46.381761
3503.815860	490122.866289	46.386765
3503.707327	490131.949185	46.391770
3503.656878	490122.030437	46.396775
3503.616224	490103.601505	46.401780
3503.630444	490088.759795	46.406785
3503.316162	490094.633841	46.411789
3503.495957	490089.743350	46.416794
3503.577361	490093.073169	46.421799
3503.575375	490087.907529	46.426804
3503.737294	490082.564041	46.431809
3503.561184	490085.782623	46.436813
3503.351377	490089.411704	46.441818
3503.811769	490095.872361	46.446823
3503.292959	490079.595493	46.451828
3503.558116	490053.622463	46.456833
3503.291897	490059.792805	46.461837
3503.758925	490044.170435	46.466842
3503.534868	490050.080881	46.471847
3503.605617	490050.880053	46.476852
3503.844623	490054.083675	46.481857
3503.963452	490054.520720	46.486861
3503.735100	490046.048161	46.491866
3503.700521	490037.089149	46.496871
3503.702297	490021.793532	46.501876
3503.635852	490015.219948	46.506881
3503.309101	490017.196180	46.511885
3503.639837	490013.092161	46.516890
3503.576033	490018.977288	46.521895
3503.322108	490020.131660	46.526900
3503.697205	490010.854649	46.531905
3503.451762	490016.565899	46.536909
3503.314004	490010.104878	46.541914
3503.656566	490015.621896	46.546919
3503.691428	490011.919170	46.551924
3503.430333	489980.255472	46.556929
3503.166430	489971.839145	46.561933
3503.402444	489972.612198	46.566938
3503.214609	489977.453356	46.571943
3503.206239	489975.631394	46.576948
3503.484190	489970.472122	46.581953
3503.512583	489979.736037	46.586957
3503.599269	489980.127517	46.591962
3503.735372	489984.461649	46.596967
3503.667556	489976.166272	46.601972
3503.859043	489970.970020	46.606977
3503.469294	489982.933667	46.611981
3503.530524	489980.746176	46.616986
3503.497951	489980.143567	46.621991
3503.018521	489973.837832	46.626996
3503.715967	489975.956068	46.632001
3503.749058	489973.671729	46.637005
3503.284095	489951.460541	46.642010
3503.237490	489948.378444	46.647015
3503.306675	489936.668042	46.652020
3503.417271	489942.930805	46.657025
3503.203612	489945.750169	46.662029
3503.427525	489921.809358	46.667034
3503.390497	489942.833760	46.672039
3503.322965	489954.999731	46.677044
3503.452633	489941.861656	46.682049
3503.279715	489952.271639	46.687053
3503.736714	489931.586056	46.692058
3503.907015	489936.016089	46.697063
3503.670523	489939.244240	46.702068
3503.930314	489941.026478	46.707073
3503.265552	489940.777026	46.712077
3503.596146	489926.442299	46.717082
3503.807173	489917.596352	46.722087
3503.236514	489903.910530	46.727092
3503.567585	489892.969063	46.732097
3503.272174	489896.206534	46.737101
3503.047801	489904.497494	46.742106
3503.512061	489911.109545	46.747111
3503.550250	489902.999969	46.752116
3503.381310	489895.986719	46.757121
3503.357905	489908.398982	46.762125
3503.393845	489903.379238	46.767130
3504.048152	489908.188600	46.772135
3503.642458	489906.328137	46.777140
3503.790561	489912.736922	46.782145
3503.676321	489904.195615	46.787149
3503.789985	489882.703244	46.792154
3503.833238	489880.214699	46.797159
3503.618007	489876.551476	46.802164
3503.699278	489863.623584	46.807169
3503.529761	489873.627895	46.812173
3503.724232	489869.292146	46.817178
3503.586699	489858.374078	46.822183
3503.634925	489842.969679	46.827188
3503.949466	489827.320583	46.832193
3503.770087	489832.008499	46.837197
3504.050664	489829.836969	46.842202
3503.918621	489836.239412	46.847207
3503.644221	489804.476225	46.852212
3503.934784	489798.251317	46.857217
3503.895091	489798.308244	46.862221
3503.631028	489799.312289	46.867226
3504.236705	489788.226062	46.872231
3503.666020	489772.362306	46.877236
3503.684361	489756.658674	46.882241
3503.772108	489760.190140	46.887245
3503.666876	489757.623753	46.892250
3503.721696	489750.271196	46.897255
3503.688228	489756.404848	46.902260
3504.068700	489720.942034	46.907265
3503.840415	489716.166594	46.912269
3503.911181	489716.307358	46.917274
3504.097060	489714.859849	46.922279
3503.759871	489700.681147	46.927284
3503.815702	489678.184728	46.932289
3504.107026	489674.289456	46.937293
3504.240990	489665.404923	46.942298
3503.936009	489662.566208	46.947303
3503.897336	489650.315550	46.952308
3504.147834	489643.387853	46.957313
3503.717711	489645.937589	46.962317
3504.038344	489626.438126	46.967322
3503.683723	489605.120749	46.972327
3503.340041	489596.666215	46.977332
3503.253430	489586.145123	46.982337
3503.517215	489598.968030	46.987341
3503.231951	489589.997780	46.992346
3503.362696	489595.801641	46.997351
3502.863929	489589.043000	47.002356
3503.280493	489584.672082	47.007361
3503.208824	489595.825980	47.012365
3503.031913	489595.195524	47.017370
3503.318780	489591.402235	47.022375
3503.219073	489589.645320	47.027380
3503.744743	489590.575200	47.032385
3503.304483	489604.370399	47.037389
3503.434435	489593.967027	47.042394
3503.510331	489599.627613	47.047399
3503.195516	489593.650266	47.052404
3503.858471	489595.166222	47.057409
3503.431324	489603.337421	47.062413
3503.502022	489603.579492	47.067418
3503.380478	489595.343087	47.072423
3503.298179	489601.079324	47.077428
3503.669890	489595.348003	47.082433
3503.747692	489594.322751	47.087437
3503.448170	489592.394827	47.092442
3503.686507	489594.079194	47.097447
3503.432868	489573.910724	47.102452
3503.724768	489556.796189	47.107457
3503.787376	489561.699165	47.112461
3503.754494	489562.514737	47.117466
3503.568924	489556.010469	47.122471
3503.807445	489555.516942	47.127476
3503.880392	489548.870515	47.132481
3503.678818	489526.414599	47.137485
3503.566700	489520.354542	47.142490
3503.571936	489509.312409	47.147495
3503.597530	489518.070512	47.152500
3503.807076	489520.012677	47.157505
3503.489034	489511.959238	47.162509
3503.482971	489510.440755	47.167514
3503.600996	489513.359703	47.172519
3503.412802	489517.795850	47.177524
3503.840082	489486.427700	47.182529
3503.606073	489488.743866	47.187533
3503.879228	489469.960821	47.192538
3503.702766	489481.941723	47.197543
3503.007711	489488.028087	47.202548
3503.642493	489480.634405	47.207553
3503.275836	489492.746658	47.212557
3503.235207	489484.092228	47.217562
3503.612384	489477.043151	47.222567
3503.414445	489480.417232	47.227572
3503.321783	489487.927832	47.232577
3503.054036	489489.135069	47.237581
3503.232810	489490.221080	47.242586
3503.323031	489486.205611	47.247591
3503.004105	489485.192411	47.252596
3503.183865	489484.151039	47.257601
3503.008107	489481.139926	47.262605
3503.087413	489487.964918	47.267610
3503.576368	489482.164382	47.272615
3503.206812	489491.390141	47.277620
3503.364242	489482.400515	47.282625
3503.065038	489486.955512	47.287629
3503.479380	489484.053723	47.292634
3503.452439	489490.743562	47.297639
3502.954833	489497.102604	47.302644
3503.672436	489488.936111	47.307649
3503.380778	489499.466409	47.312653
3503.122191	489498.190432	47.317658
3503.519725	489507.142993	47.322663
3503.312961	489502.364096	47.327668
3503.412877	489497.587373	47.332673
3503.274266	489501.914389	47.337677
3503.264308	489504.397734	47.342682
3503.360421	489499.368371	47.347687
3503.153640	489501.578935	47.352692
3503.427838	489494.191603	47.357697
3503.294342	489504.696899	47.362701
3503.365617	489508.180368	47.367706
3503.526290	489501.874596	47.372711
3503.402521	489511.567979	47.377716
3503.662212	489510.969808	47.382721
3503.205514	489514.536726	47.387725
3503.354596	489503.319908	47.392730
3503.716002	489506.554927	47.397735
3502.979353	489503.176637	47.402740
3503.029232	489512.488035	47.407745
3503.222214	489505.974565	47.412749
3503.295286	489503.886443	47.417754
3503.557884	489502.680033	47.422759
3503.239650	489510.428871	47.427764
3503.503026	489505.828907	47.432769
3503.525034	489505.774786	47.437773
3503.547402	489507.392000	47.442778
3503.587212	489508.854513	47.447783
3503.435229	489513.183640	47.452788
3503.705417	489506.809912	47.457793
3503.819840	489502.841269	47.462797
3503.506831	489477.667902	47.467802
3503.409339	489471.605518	47.472807
3503.219306	489468.697957	47.477812
3503.256216	489468.540184	47.482817
3503.592542	489463.878031	47.487821
3503.256474	489467.628485	47.492826
3503.711883	489467.708454	47.497831
3503.326607	489470.048532	47.502836
3503.328341	489473.492350	47.507841
3503.588758	489470.209702	47.512845
3503.633757	489479.319294	47.517850
3503.554082	489480.446156	47.522855
3503.322121	489469.846677	47.527860
3503.832430	489466.828420	47.532865
3503.681116	489479.007942	47.537869
3503.393663	489462.592672	47.542874
3503.549815	489441.295674	47.547879
3503.309831	489444.119274	47.552884
3503.459038	489432.395910	47.557889
3503.494183	489444.090147	47.562893
3503.593330	489440.478445	47.567898
3503.605277	489430.346876	47.572903
3503.255895	489450.154988	47.577908
3503.338369	489431.604637	47.582913
3503.402832	489444.459154	47.587917
3503.116273	489445.365476	47.592922
3503.736664	489427.489825	47.597927
3503.363087	489439.957745	47.602932
3503.696907	489439.094613	47.607937
3503.704482	489449.830884	47.612941
3503.656298	489443.760698	47.617946
3503.886914	489410.296272	47.622951
3503.329102	489405.319594	47.627956
3503.664626	489400.606904	47.632961
3503.569817	489395.860933	47.637965
3503.500279	489398.404357	47.642970
3503.489510	489395.468449	47.647975
3503.347924	489405.569891	47.652980
3503.482214	489384.478878	47.657985
3503.599110	489403.352315	47.662989
3503.077854	489400.598392	47.667994
3503.427150	489392.743314	47.672999
3503.189615	489398.504149	47.678004
3503.518996	489399.617010	47.683009
3503.418102	489400.291394	47.688013
3503.391830	489404.701974	47.693018
3503.797205	489399.876946	47.698023
3503.382436	489395.941275	47.703028
3503.796678	489385.594150	47.708033
3503.473815	489375.667417	47.713037
3503.825151	489372.319732	47.718042
3504.037013	489363.473392	47.723047
3503.681163	489360.794617	47.728052
3503.739299	489371.522942	47.733057
3503.613493	489352.650893	47.738061
3503.765225	489332.671335	47.743066
3503.667381	489329.040099	47.748071
3503.432979	489337.332893	47.753076
3503.652488	489329.245059	47.758081
3503.547064	489339.948605	47.763085
3503.663811	489331.826366	47.768090
3503.557067	489333.767895	47.773095
3503.422091	489342.399513	47.778100
3503.503588	489321.215476	47.783105
3503.650037	489314.304104	47.788109
3503.500521	489296.853912	47.793114
3503.584199	489290.408292	47.798119
3503.561805	489288.943022	47.803124
3503.358292	489282.086953	47.808129
3503.388541	489287.906794	47.813133
3503.454626	489285.009371	47.818138
3503.707320	489293.427791	47.823143
3503.503882	489290.572969	47.828148
3503.910569	489285.342514	47.833153
3503.501675	489287.382453	47.838157
3503.121172	489291.038668	47.843162
3503.584570	489286.609630	47.848167
3503.641454	489283.409768	47.853172
3503.505770	489254.814602	47.858177
3503.569632	489252.120122	47.863181
3503.582013	489250.193511	47.868186
3503.704534	489259.594851	47.873191
3503.229745	489249.742713	47.878196
3503.580495	489245.382120	47.883201
3503.605269	489256.014485	47.888205
3503.232764	489250.400689	47.893210
3503.391682	489251.185960	47.898215
3503.272786	489255.712512	47.903220
3503.573268	489244.269014	47.908225
3503.465530	489244.235400	47.913229
3503.512250	489253.901968	47.918234
3503.534569	489243.566064	47.923239
3502.984781	489240.360786	47.928244
3503.185944	489245.191296	47.933249
3503.282532	489247.353940	47.938253
3503.454537	489256.798108	47.943258
3503.691921	489255.494370	47.948263
3503.639257	489252.413116	47.953268
3503.731702	489229.201288	47.958273
3503.695085	489223.331798	47.963277
3503.657138	489215.993694	47.968282
3503.903883	489214.435229	47.973287
3503.587721	489219.043619	47.978292
3503.488399	489221.135933	47.983297
3503.415125	489228.390328	47.988301
3503.694848	489212.948822	47.993306
3503.795049	489183.050037	47.998311
3503.673154	489183.575801	48.003316
3504.022376	489178.050504	48.008321
3503.688706	489182.914916	48.013325
3503.642887	489172.944286	48.018330
3503.722235	489171.159030	48.023335
3503.230029	489158.574543	48.028340
3503.584642	489132.535453	48.033345
3503.705049	489138.493038	48.038349
3503.649401	489139.616122	48.043354
3503.837928	489143.334372	48.048359
3503.717044	489135.047011	48.053364
3503.657502	489132.574615	48.058369
3503.206229	489140.901774	48.063373
3503.148676	489141.113474	48.068378
3503.425565	489137.878814	48.073383
3503.204778	489146.118891	48.078388
3503.400208	489142.542562	48.083393
3503.610097	489139.217194	48.088397
3503.325836	489137.590705	48.093402
3503.666550	489125.330388	48.098407
3503.330291	489119.558876	48.103412
3503.433173	489101.106272	48.108417
3503.769583	489099.482976	48.113421
3503.570483	489102.401464	48.118426
3503.903199	489093.080051	48.123431
3503.618194	489098.595234	48.128436
3503.594062	489097.231522	48.133441
3503.597860	489099.763395	48.138445
3503.625961	489089.527790	48.143450
3503.696259	489077.715379	48.148455
3503.488282	489089.650862	48.153460
3503.566879	489071.911159	48.158465
3503.532367	489074.246493	48.163469
3503.499209	489071.364723	48.168474
3503.791384	489063.012043	48.173479
3503.755343	489064.182682	48.178484
3503.836212	489060.725744	48.183489
3503.753872	489056.079015	48.188493
3503.635044	489040.244517	48.193498
3503.430797	489023.106619	48.198503
3503.283553	489025.003931	48.203508
3503.526185	489032.208469	48.208513
3503.354573	489024.182325	48.213517
3503.537191	489027.040490	48.218522
3503.895965	489020.652596	48.223527
3503.812321	489021.780112	48.228532
3503.526780	489034.436983	48.233537
3503.576586	489014.422549	48.238541
3503.278579	489000.389072	48.243546
3503.668826	488987.462393	48.248551
3503.556959	488991.785299	48.253556
3503.566356	488996.595533	48.258561
3503.160054	489000.407830	48.263565
3503.343450	489002.404832	48.268570
3503.659819	488986.197605	48.273575
3503.461998	488990.027601	48.278580
3503.423992	488994.490781	48.283585
3503.270297	489003.632009	48.288589
3503.570979	488990.618188	48.293594
3503.727147	488992.720795	48.298599
3503.611377	488999.475498	48.303604
3503.817665	488981.664878	48.308609
3503.803178	488961.255352	48.313613
3503.587238	488958.351806	48.318618
3503.660862	488945.930990	48.323623
3503.321719	488946.744347	48.328628
3503.267701	488948.880180	48.333633
3503.396967	488952.810434	48.338637
3503.307121	488955.103878	48.343642
3503.613344	488949.838560	48.348647
3503.196429	488953.905792	48.353652
3503.553397	488946.454514	48.358657
3503.699845	488953.471687	48.363661
3503.719764	488959.749110	48.368666
3503.681007	488946.991509	48.373671
3503.349679	488928.050219	48.378676
3503.514122	488913.183837	48.383681
3503.561887	488919.051674	48.388685
3503.521107	488917.589280	48.393690
3503.722053	488918.317272	48.398695
3503.431399	488924.795745	48.403700
3503.702856	488921.561907	48.408705
3503.685543	488925.059486	48.413709
3503.672786	488916.906888	48.418714
3503.710430	488918.167189	48.423719
3503.463954	488892.526674	48.428724
3503.500865	488870.842679	48.433729
3503.315638	488885.661741	48.438733
3503.491587	488880.265045	48.443738
3503.832135	488865.725340	48.448743
3503.668761	488878.768206	48.453748
3503.633639	488875.380217	48.458753
3503.601860	488883.387935	48.463757
3503.462088	488877.129442	48.468762
3503.618674	488877.965747	48.473767
3503.646108	488858.613132	48.478772
3503.635808	488839.772962	48.483777
3503.580654	488834.767331	48.488781
3503.620772	488837.344148	48.493786
3503.791349	488829.010585	48.498791
3503.333749	488841.542830	48.503796
3503.799730	488839.848382	48.508801
3503.746055	488837.982821	48.513805
3503.634231	488822.298982	48.518810
3503.604300	488798.700765	48.523815
3503.644361	488790.286513	48.528820
3503.781391	488786.567398	48.533825
3503.550633	488789.338986	48.538829
3503.238710	488793.541608	48.543834
3503.822963	488788.637502	48.548839
3503.543357	488790.403808	48.553844
3503.708567	488790.833552	48.558849
3503.483996	488766.506307	48.563853
3503.353718	488763.589191	48.568858
3503.585972	488750.434070	48.573863
3503.303073	488764.154360	48.578868
3503.480293	488756.832719	48.583873
3503.532153	488753.329660	48.588877
3503.201526	488764.980832	48.593882
3503.294630	488759.445245	48.598887
3503.424414	488764.489762	48.603892
3503.319142	488754.072455	48.608897
3503.521617	488755.965168	48.613901
3503.410076	488762.010184	48.618906
3503.354052	488758.321577	48.623911
3503.441958	488762.562310	48.628916
3503.634137	488761.063083	48.633921
3503.570943	488765.074446	48.638925
3503.671919	488758.372659	48.643930
3503.538299	488757.988583	48.648935
3503.231064	488769.332154	48.653940
3503.386245	488764.698461	48.658945
3503.523952	488762.802642	48.663949
3503.237635	488769.989585	48.668954
3503.312194	488766.280340	48.673959
3503.456820	488776.691432	48.678964
3503.659456	488743.838048	48.683969
3503.505519	488740.367514	48.688973
3503.374072	488737.957082	48.693978
3503.334162	488725.047562	48.698983
3503.423321	488720.424294	48.703988
3503.175281	488725.325938	48.708993
3502.954713	488716.142442	48.713997
3503.344541	488715.878231	48.719002
3503.505755	488728.059490	48.724007
3503.438116	488721.080439	48.729012
3503.454951	488717.785511	48.734017
3503.102270	488723.919304	48.739021
3503.388485	488723.013015	48.744026
3503.463219	488718.088124	48.749031
3503.378079	488721.799063	48.754036
3503.507060	488728.059325	48.759041
3503.208334	488725.877932	48.764045
3503.564215	488720.706003	48.769050
3503.595525	488720.802361	48.774055
3503.521967	488737.984456	48.779060
3503.128202	488729.132243	48.784065
3503.330861	488731.379482	48.789069
3503.075016	488727.215948	48.794074
3503.382165	488732.890894	48.799079
3503.347712	488724.690991	48.804084
3503.487951	488728.771509	48.809089
3503.302314	488737.563362	48.814093
3503.156852	488733.281083	48.819098
3503.595495	488732.806555	48.824103
3503.476197	488748.071157	48.829108
3503.500889	488736.670944	48.834113
3503.540933	488731.447637	48.839117
3503.298383	488743.540754	48.844122
3503.402644	488734.711127	48.849127
3503.376013	488736.184202	48.854132
3503.513769	488744.975587	48.859137
3503.754078	488742.405095	48.864141
3503.521116	488719.396023	48.869146
3503.622796	488700.234112	48.874151
3503.151842	488708.311320	48.879156
3503.432659	488690.893848	48.884161
3503.331439	488701.242539	48.889165
3503.296902	488703.932475	48.894170
3503.582374	488693.706627	48.899175
3503.365322	488711.164679	48.904180
3503.641884	488708.740403	48.909185
3503.617686	488698.614154	48.914189
3503.594950	488698.617753	48.919194
3503.449670	488701.021291	48.924199
3503.200502	488714.280432	48.929204
3503.444612	488718.293884	48.934209
3503.674374	488714.610747	48.939213
3503.362953	488711.722254	48.944218
3503.346150	488708.432641	48.949223
3503.512790	488708.912812	48.954228
3503.778404	488708.516282	48.959233
3503.527324	488678.773522	48.964237
3503.152555	488678.174307	48.969242
3503.419533	488660.201840	48.974247
3503.004564	488675.563885	48.979252
3503.345979	488673.635860	48.984257
3503.403623	488666.434385	48.989261
3503.246677	488676.386693	48.994266
3503.500223	488672.750440	48.999271
3503.511050	488667.481083	49.004276
3503.328355	488668.016471	49.009281
3503.331894	488676.322597	49.014285
3503.396415	488679.908588	49.019290
3503.407008	488674.993824	49.024295
3503.302687	488682.759840	49.029300
3503.378751	488674.238545	49.034305
3503.494720	488673.308512	49.039309
3503.614944	488672.580409	49.044314
3503.384387	488667.450506	49.049319
3503.676026	488671.304504	49.054324
3503.321540	488668.777364	49.059329
3503.415295	488673.017192	49.064333
3503.418274	488668.559484	49.069338
3503.834253	488669.506751	49.074343
3503.576910	488675.524189	49.079348
3503.635875	488668.221205	49.084353
3503.919359	488657.843700	49.089357
3503.518089	488642.002859	49.094362
3503.751654	488630.974771	49.099367
3503.632716	488642.845812	49.104372
3503.542562	488640.226238	49.109377
3503.784618	488636.591794	49.114381
3503.741273	488626.671134	49.119386
3503.830576	488600.622595	49.124391
3503.603505	488594.327155	49.129396
3503.397494	488596.639004	49.134401
3503.805457	488602.450007	49.139405
3503.399098	488591.472392	49.144410
3503.811917	488596.573519	49.149415
3503.671995	488592.442284	49.154420
3503.651550	488568.082519	49.159425
3503.569001	488564.701970	49.164429
3503.610107	488555.021179	49.169434
3503.607954	488560.238557	49.174439
3503.757704	488550.540591	49.179444
3503.691885	488554.096556	49.184449
3503.931651	488562.162792	49.189453
3503.615182	488542.864210	49.194458
3503.713185	488519.144121	49.199463
3503.658450	488509.073247	49.204468
3503.494309	488504.287359	49.209473
3503.709829	488509.520996	49.214477
3503.655269	488500.767014	49.219482
3503.943306	488507.863276	49.224487
3503.351314	488509.729633	49.229492
3503.579488	488505.286943	49.234497
3503.864551	488486.501038	49.239501
3503.876766	488477.229981	49.244506
3503.441272	488475.576686	49.249511
3503.445713	488482.515177	49.254516
3503.593232	488470.183671	49.259521
3504.006871	488468.345511	49.264525
3503.567357	488472.467068	49.269530
3503.737801	488444.075541	49.274535
3503.539261	488443.296510	49.279540
3503.807551	488435.048630	49.284545
3503.742476	488433.995248	49.289549
3503.576965	488431.286254	49.294554
3503.841553	488415.036070	49.299559
3503.699332	488417.236555	49.304564
3503.790899	488406.433386	49.309569
3503.651429	488394.653703	49.314573
3503.519288	488394.877200	49.319578
3503.300708	488390.910307	49.324583
3503.352961	488392.826801	49.329588
3503.536791	488392.899053	49.334593
3503.643517	488388.880742	49.339597
3503.612926	488381.794407	49.344602
3503.765382	488389.519958	49.349607
3503.847179	488381.808045	49.354612
3503.737328	488359.336239	49.359617
3503.612257	488357.076703	49.364621
3503.443212	488344.845802	49.369626
3503.668862	488342.328225	49.374631
3503.516529	488346.556372	49.379636
3503.676089	488351.748247	49.384641
3503.780258	488349.705734	49.389645
3503.529487	488331.206973	49.394650
3503.577413	488304.860657	49.399655
3503.487199	488317.841694	49.404660
3503.274011	488304.756670	49.409665
3503.655715	488304.139178	49.414669
3503.532088	488324.064742	49.419674
3503.421518	488312.179138	49.424679
3503.555790	488312.005966	49.429684
3503.398435	488312.132146	49.434689
3503.514044	488313.329514	49.439693
3503.526868	488311.048178	49.444698
3503.705810	488306.815829	49.449703
3503.564291	488309.218822	49.454708
3503.489766	488292.414315	49.459713
3503.853982	488267.334894	49.464717
3503.531270	488269.209364	49.469722
3503.496491	488268.151184	49.474727
3503.613447	488257.495871	49.479732
3503.424234	488252.713881	49.484737
3503.371285	488272.223116	49.489741
3503.261500	488268.644214	49.494746
3503.604544	488265.196343	49.499751
3503.515207	488286.028256	49.504756
3503.545657	488271.283851	49.509761
3503.821025	488269.720785	49.514765
3503.471905	488255.897439	49.519770
3503.525281	488226.359101	49.524775
3503.412536	488238.026810	49.529780
3503.439685	488227.335024	49.534785
3503.655172	488231.353104	49.539789
3503.417228	488232.353101	49.544794
3503.640545	488234.951696	49.549799
3503.513820	488229.501352	49.554804
3503.332654	488238.799246	49.559809
3503.838649	488235.984086	49.564813
3503.361142	488250.191373	49.569818
3503.455259	488234.575798	49.574823
3503.784774	488220.290599	49.579828
3503.606283	488219.204480	49.584833
3503.267786	488202.897482	49.589837
3503.432295	488186.662920	49.594842
3503.797077	488178.450330	49.599847
3503.449017	488189.294182	49.604852
3503.430777	488185.650142	49.609857
3503.650795	488178.372165	49.614861
3503.355895	488195.083220	49.619866
3503.459555	488180.833690	49.624871
3503.419661	488183.727155	49.629876
3503.387479	488197.408227	49.634881
3503.395965	488202.016201	49.639885
3503.288387	488192.561331	49.644890
3503.581780	488190.590197	49.649895
3503.442519	488192.739588	49.654900
3503.593931	488194.133912	49.659905
3503.766312	488186.863467	49.664909
3503.291409	488163.891959	49.669914
3503.590669	488159.995123	49.674919
3503.541524	488159.496378	49.679924
3503.436026	488158.601325	49.684929
3503.486399	488159.251843	49.689933
3503.492219	488155.553343	49.694938
3503.942805	488151.227372	49.699943
3503.695516	488161.954008	49.704948
3503.496818	488161.732161	49.709953
3503.583144	488155.387039	49.714957
3503.274165	488141.202701	49.719962
3503.455839	488140.110301	49.724967
3503.563051	488124.593870	49.729972
3503.689050	488107.200332	49.734977
3503.655399	488112.979984	49.739981
3503.371581	488121.129166	49.744986
3503.580250	488110.155363	49.749991
3503.487830	488121.414715	49.754996
3503.436938	488118.181039	49.760001
3503.534053	488119.229387	49.765005
3503.443874	488113.165409	49.770010
3503.712630	488113.072284	49.775015
3503.793332	488113.667358	49.780020
3503.259016	488100.632949	49.785025
3503.500329	488080.080734	49.790029
3503.165241	488075.068496	49.795034
3503.620205	488067.905297	49.800039
3503.555691	488073.284623	49.805044
3503.288687	488087.610715	49.810049
3503.539845	488070.501274	49.815053
3503.638639	488079.451084	49.820058
3503.584355	488062.997738	49.825063
3503.642449	488074.739850	49.830068
3503.480916	488073.600389	49.835073
3503.777793	488080.594110	49.840077
3503.349688	488084.207426	49.845082
3503.469788	488063.725005	49.850087
3503.569224	488079.614053	49.855092
3503.367319	488057.662958	49.860097
3503.639696	488039.739701	49.865101
3503.274680	488036.707618	49.870106
3503.430999	488027.818781	49.875111
3503.375552	488033.703206	49.880116
3503.323381	488034.623198	49.885121
3503.315830	488034.725702	49.890125
3503.282413	488036.351859	49.895130
3503.728936	488032.482374	49.900135
3503.781841	488035.310541	49.905140
3503.285541	488042.227036	49.910145
3503.415483	488037.850416	49.915149
3503.218272	488041.072680	49.920154
3503.621814	488041.869989	49.925159
3503.201916	488043.810494	49.930164
3503.379988	488040.895180	49.935169
3503.573136	488036.660526	49.940173
3503.285040	488046.228677	49.945178
3503.491460	488040.877579	49.950183
3503.547875	488037.120406	49.955188
3503.580113	488035.494447	49.960193
3503.301886	488045.618212	49.965197
3503.518678	488037.530256	49.970202
3503.519342	488028.666022	49.975207
3503.680308	488021.599928	49.980212
3503.732178	488003.204967	49.985217
3503.860708	488009.516191	49.990221
3503.365846	488002.857662	49.995226
3503.522172	487999.337952	50.000231
3503.576714	488007.281744	50.005236
3503.126622	488009.075068	50.010241
3503.389687	488007.159361	50.015245
3503.387074	488018.455232	50.020250
3503.814343	488004.508986	50.025255
3503.490419	488007.903241	50.030260
3503.545290	487993.509325	50.035265
3503.620452	487974.958698	50.040269
3503.538113	487965.246464	50.045274
3503.436927	487965.414420	50.050279
3503.733504	487970.331482	50.055284
3503.597511	487962.147297	50.060289
3503.525843	487964.437988	50.065293
3503.459106	487961.156137	50.070298
3503.717808	487958.886548	50.075303
3503.343541	487966.391611	50.080308
3503.443439	487962.272984	50.085313
3503.960849	487960.519680	50.090317
3503.823252	487935.772398	50.095322
3503.973145	487922.376458	50.100327
3503.977820	487925.161612	50.105332
3503.512835	487921.030955	50.110337
3503.758326	487906.809454	50.115341
3503.381252	487900.841407	50.120346
3503.393016	487881.490269	50.125351
3503.451345	487877.682109	50.130356
3503.398222	487879.412701	50.135361
3503.677442	487869.795228	50.140365
3503.390624	487882.807638	50.145370
3503.320510	487883.375904	50.150375
3503.434407	487876.722416	50.155380
3503.446653	487888.927763	50.160385
3503.530790	487884.001169	50.165389
3503.476948	487883.655117	50.170394
3503.642509	487875.321927	50.175399
3503.511019	487885.321279	50.180404
3503.494752	487882.487311	50.185409
3503.637088	487874.208443	50.190413
3503.544879	487869.005803	50.195418
3503.595921	487864.844224	50.200423
3503.374709	487855.052578	50.205428
3503.501149	487860.097866	50.210433
3503.597204	487844.076442	50.215437
3503.580057	487866.315682	50.220442
3503.538092	487850.822605	50.225447
3503.216216	487857.762250	50.230452
3503.074874	487861.482241	50.235457
3503.449231	487859.650233	50.240461
3503.320416	487866.863276	50.245466
3503.337336	487859.009447	50.250471
3503.416566	487858.034529	50.255476
3502.893968	487857.002777	50.260481
3503.361666	487860.930420	50.265485
3503.266196	487867.631665	50.270490
3503.539566	487854.216160	50.275495
3503.147239	487860.913677	50.280500
3503.101403	487864.264003	50.285505
3503.499262	487852.145789	50.290509
3503.332721	487869.039454	50.295514
3503.138830	487865.017894	50.300519
3503.425912	487871.658673	50.305524
3503.279372	487864.894387	50.310529
3503.533769	487875.795152	50.315533
3503.405431	487871.206054	50.320538
3503.715481	487865.838527	50.325543
3503.576570	487866.822889	50.330548
3503.396783	487887.011053	50.335553
3503.743137	487873.482721	50.340557
3503.424821	487875.660450	50.345562
3503.529083	487865.564102	50.350567
3503.486631	487874.232418	50.355572
3503.557414	487850.921015	50.360577
3503.455411	487836.501122	50.365581
3503.502209	487818.512005	50.370586
3503.478955	487818.667645	50.375591
3503.495914	487826.262885	50.380596
3503.365002	487823.041806	50.385601
3503.542790	487819.923892	50.390605
3503.544515	487824.330416	50.395610
3503.323754	487824.618579	50.400615
3503.536692	487819.519652	50.405620
3503.668563	487834.694639	50.410625
3503.762160	487833.160269	50.415629
3503.393208	487828.811803	50.420634
3503.308763	487818.491993	50.425639
3503.555071	487825.189885	50.430644
3503.524613	487817.900707	50.435649
3503.717287	487800.141780	50.440653
3503.434082	487788.688355	50.445658
3503.467447	487791.367688	50.450663
3503.406026	487786.362770	50.455668
3503.287758	487783.291644	50.460673
3503.600106	487776.657407	50.465677
3503.038804	487787.737804	50.470682
3503.336584	487779.434326	50.475687
3503.281028	487788.965852	50.480692
3503.216966	487789.229248	50.485697
3503.847875	487774.085630	50.490701
3503.661913	487779.889457	50.495706
3503.450052	487788.533937	50.500711
3503.522705	487781.380405	50.505716
3503.517409	487798.957787	50.510721
3503.600719	487782.938325	50.515725
3503.548893	487767.193474	50.520730
3503.751929	487753.991627	50.525735
3503.663675	487724.120321	50.530740
3503.668554	487697.476046	50.535745
3503.624813	487648.906584	50.540749
3503.541636	487583.171735	50.545754
3503.224265	487520.614196	50.550759
3503.316450	487443.352781	50.555764
3503.050397	487349.887740	50.560769
3502.804143	487257.128268	50.565773
3502.417932	487166.568609	50.570778
3502.935161	487041.319146	50.575783
3502.798983	486935.927647	50.580788
3502.490778	486797.130155	50.585793
3502.320227	486646.962975	50.590797
3501.868484	486504.082905	50.595802
3501.915858	486340.252319	50.600807
3501.858142	486176.436937	50.605812
3501.260629	486006.271956	50.610817
3501.287960	485827.546799	50.615821
3500.916103	485641.182968	50.620826
3500.818915	485433.041158	50.625831
3500.806165	485237.497995	50.630836
3500.300810	485025.515483	50.635841
3499.886268	484800.648440	50.640845
3499.774793	484579.023852	50.645850
3499.509365	484340.297298	50.650855
3499.162508	484111.003901	50.655860
3498.593137	483850.433064	50.660865
3498.618658	483596.908298	50.665869
3497.779300	483352.940527	50.670874
3497.334740	483078.305456	50.675879
3497.505949	482807.875774	50.680884
3497.346472	482550.110603	50.685889
3496.987779	482255.842303	50.690893
3496.437390	481955.773006	50.695898
3496.237116	481659.494592	50.700903
3495.416791	481373.747659	50.705908
3495.006140	481060.417698	50.710913
3494.871282	480754.285133	50.715917
3494.478288	480445.857672	50.720922
3494.125070	480113.248071	50.725927
3493.709790	479790.169338	50.730932
3493.046317	479462.715840	50.735937
3492.809799	479107.115164	50.740941
3492.457788	478783.452515	50.745946
3491.814929	478433.326331	50.750951
3491.467748	478083.045872	50.755956
3491.234246	477727.318604	50.760961
3490.820838	477362.186931	50.765965
3490.267378	476997.526837	50.770970
3489.814495	476615.308247	50.775975
3489.386914	476246.661371	50.780980
3488.557830	475867.630317	50.785985
3488.274275	475481.105900	50.790989
3487.548633	475103.919437	50.795994
3487.019364	474713.719079	50.800999
3486.008949	474337.931857	50.806004
3485.488387	473940.568246	50.811009
3485.454969	473553.257778	50.816013
3484.892790	473161.359979	50.821018
3484.352116	472763.469635	50.826023
3484.095443	472366.946034	50.831028
3483.195821	471956.575645	50.836033
3482.384280	471546.943535	50.841037
3481.487913	471145.275872	50.846042
3481.357757	470718.790003	50.851047
3480.833969	470310.862191	50.856052
3480.025365	469899.980130	50.861057
3479.636825	469475.436006	50.866061
3479.000179	469065.422824	50.871066
3478.759912	468641.548043	50.876071
3477.913783	468216.036526	50.881076
3477.150344	467798.159543	50.886081
3476.713064	467357.304096	50.891085
3475.858477	466948.754282	50.896090
3475.330904	466511.495481	50.901095
3474.767402	466086.910270	50.906100
3473.653850	465661.287884	50.911105
3473.332157	465216.211283	50.916109
3472.775236	464793.069694	50.921114
3472.131381	464366.535732	50.926119
3471.669480	463922.214921	50.931124
3470.875646	463487.826597	50.936129
3470.562871	463043.818983	50.941133
3469.391040	462618.297240	50.946138
3468.915119	462168.667864	50.951143
3468.187886	461735.298682	50.956148
3467.628452	461297.988916	50.961153
3467.085534	460848.951343	50.966157
3466.186430	460421.618797	50.971162
3465.627153	459978.398800	50.976167
3464.864637	459528.607907	50.981172
3464.034547	459093.883597	50.986177
3463.846356	458647.534548	50.991181
3463.179930	458223.673111	50.996186
3462.766963	457765.421036	51.001191
3461.830720	457308.053844	51.006196
3460.914402	456873.350141	51.011201
3460.649881	456422.757728	51.016205
3460.147752	455966.105988	51.021210
3459.075691	455518.717599	51.026215
3458.575102	455076.201820	51.031220
3457.654177	454619.741035	51.036225
3456.807316	454157.069544	51.041229
3456.223475	453730.928074	51.046234
3456.099439	453265.891664	51.051239
3455.355222	452817.941202	51.056244
3454.318268	452367.440474	51.061249
3453.477220	451914.362844	51.066253
3453.051071	451476.179416	51.071258
3452.313085	451023.575278	51.076263
3451.635381	450575.824080	51.081268
3450.963392	450118.472554	51.086273
3450.686793	449681.195452	51.091277
3449.120053	449231.173692	51.096282
3448.637480	448770.010352	51.101287
3448.168858	448338.016056	51.106292
3447.034367	447883.890784	51.111297
3446.526286	447450.008584	51.116301
3445.697287	447005.054552	51.121306
3445.038228	446564.886707	51.126311
3444.438035	446119.372251	51.131316
3443.557729	445688.916925	51.136321
3443.147429	445229.347549	51.141325
3442.102523	444806.617029	51.146330
3441.460250	444363.208025	51.151335
3440.845741	443920.446257	51.156340
3439.716896	443492.071618	51.161345
3439.288124	443053.883549	51.166349
3438.964630	442621.000738	51.171354
3438.002623	442185.673034	51.176359
3437.283396	441740.603479	51.181364
3436.262566	441302.375749	51.186369
3436.183808	440868.813806	51.191373
3435.245723	440445.685360	51.196378
3434.444777	440017.552839	51.201383
3434.053877	439572.645673	51.206388
3433.084053	439136.909449	51.211393
3432.735951	438704.037212	51.216397
3431.776044	438274.173382	51.221402
3431.169669	437836.605236	51.226407
3430.114064	437410.371678	51.231412
3429.365768	436980.985137	51.236417
3429.240899	436547.100777	51.241421
3428.192672	436125.540669	51.246426
3427.510601	435696.426299	51.251431
3426.945976	435267.768426	51.256436
3426.033497	434830.983235	51.261441
3425.598709	434400.462185	51.266445
3424.635690	433974.485853	51.271450
3423.852595	433551.089082	51.276455
3423.266198	433134.585674	51.281460
3422.610420	432708.082630	51.286465
3422.245400	432273.731538	51.291469
3421.018060	431851.037106	51.296474
3420.286950	431426.733797	51.301479
3419.542606	431002.882687	51.306484
3418.748900	430595.004364	51.311489
3418.606614	430171.120691	51.316493
3417.767667	429755.897838	51.321498
3416.761842	429331.019767	51.326503
3416.328630	428912.748345	51.331508
3414.994316	428497.914037	51.336513
3414.661095	428079.334244	51.341517
3413.743216	427669.271527	51.346522
3412.953567	427263.550267	51.351527
3412.290036	426857.777486	51.356532
3411.658432	426443.485657	51.361537
3411.105255	426032.451216	51.366541
3410.203869	425628.449787	51.371546
3409.706168	425205.482598	51.376551
3408.898470	424803.130230	51.381556
3407.980596	424401.373461	51.386561
3407.454570	423990.354417	51.391565
3406.885104	423590.130692	51.396570
3406.082922	423189.582297	51.401575
3405.261374	422777.905923	51.406580
3404.483125	422384.758758	51.411585
3404.031086	421974.256533	51.416589
3403.274404	421585.133255	51.421594
3402.483450	421176.476234	51.426599
3402.017111	420771.216510	51.431604
3401.125145	420382.809003	51.436609
3400.557494	419983.701159	51.441613
3400.143437	419581.464184	51.446618
3398.734659	419182.401702	51.451623
3398.317496	418774.768178	51.456628
3397.591041	418389.253708	51.461633
3396.844990	417986.004876	51.466637
3396.079143	417602.010176	51.471642
3395.600862	417200.359154	51.476647
3394.701963	416806.111132	51.481652
3394.110929	416431.117333	51.486657
3393.465058	416018.424730	51.491661
3392.572887	415635.516058	51.496666
3391.725731	415245.760771	51.501671
3391.237978	414862.930350	51.506676
3390.298471	414473.357119	51.511681
3389.980756	414081.444470	51.516685
3389.399473	413692.363121	51.521690
3388.955467	413296.394611	51.526695
3387.893990	412913.959634	51.531700
3386.968149	412539.781603	51.536705
3386.196820	412140.825609	51.541709
3385.406117	411764.278717	51.546714
3384.778831	411377.283068	51.551719
3384.110423	411003.908872	51.556724
3383.605541	410626.870410	51.561729
3382.774586	410228.508053	51.566733
3381.853625	409876.733710	51.571738
3381.494288	409478.388479	51.576743
3381.001318	409108.622237	51.581748
3380.101891	408728.674578	51.586753
3379.455427	408345.505579	51.591757
3378.617194	407965.818243	51.596762
3377.729893	407581.127522	51.601767
3377.153864	407218.365511	51.606772
3376.599072	406836.077980	51.611777
3375.903090	406455.891993	51.616781
3375.142630	406094.365779	51.621786
3374.814436	405720.974517	51.626791
3373.943722	405343.776034	51.631796
3373.178161	404972.300243	51.636801
3372.584423	404593.422298	51.641805
3371.928765	404221.742302	51.646810
3371.264699	403829.929486	51.651815
3370.636209	403456.304506	51.656820
3369.647729	403093.203818	51.661825
3369.601205	402708.497860	51.666829
3368.279937	402342.543635	51.671834
3367.648752	401966.080187	51.676839
3367.323597	401588.140498	51.681844
3366.301236	401217.627116	51.686849
3365.826984	400839.880126	51.691853
3365.133740	400475.279564	51.696858
3364.204079	400104.077836	51.701863
3363.730047	399731.706768	51.706868
3362.705077	399368.366364	51.711873
3362.326187	398993.480669	51.716877
3361.549265	398629.889471	51.721882
3360.913474	398261.747036	51.726887
3360.356103	397887.334510	51.731892
3359.303865	397521.740931	51.736897
3358.651280	397156.308913	51.741901
3358.277915	396792.684522	51.746906
3357.100608	396423.793796	51.751911
3356.739956	396051.668322	51.756916
3355.847106	395703.215157	51.761921
3355.641470	395326.353934	51.766925
3354.431106	394962.079363	51.771930
3353.969542	394608.843392	51.776935
3353.424434	394228.566028	51.781940
3352.764729	393871.463885	51.786945
3352.133715	393507.565172	51.791949
3351.311195	393136.701105	51.796954
3350.750061	392779.470296	51.801959
3349.819675	392415.276834	51.806964
3349.141872	392060.980934	51.811969
3348.394760	391692.225162	51.816973
3347.660562	391341.210754	51.821978
3346.844496	390968.847748	51.826983
3345.968079	390612.076757	51.831988
3345.262885	390265.191489	51.836993
3345.121780	389908.831048	51.841997
3344.442029	389549.958617	51.847002
3343.572805	389188.646048	51.852007
3342.875777	388830.048775	51.857012
3342.271215	388482.443601	51.862017
3341.763556	388118.876213	51.867021
3341.125015	387778.516639	51.872026
3340.531929	387406.589582	51.877031
3339.635610	387047.828023	51.882036
3338.607798	386694.245846	51.887041
3337.737255	386339.440174	51.892045
3337.155111	385982.576491	51.897050
3336.837745	385636.678647	51.902055
3335.737426	385295.656816	51.907060
3335.242667	384948.636192	51.912065
3334.662847	384593.335349	51.917069
3333.771751	384245.073838	51.922074
3332.698645	383899.533555	51.927079
3332.316043	383557.695585	51.932084
3331.915311	383214.255165	51.937089
3331.198182	382861.604432	51.942093
3330.253397	382520.786905	51.947098
3329.622626	382178.263542	51.952103
3328.953291	381832.233484	51.957108
3328.439556	381493.169695	51.962113
3327.878383	381132.441439	51.967117
3327.034345	380802.732255	51.972122
3326.082836	380458.260374	51.977127
3325.639353	380105.693446	51.982132
3325.136541	379772.233587	51.987137
3324.470117	379419.950011	51.992141
3323.765678	379077.868454	51.997146
3323.203533	378738.253989	52.002151
3322.215345	378390.005239	52.007156
3321.311998	378052.270104	52.012161
3321.077347	377704.404819	52.017165
3320.218287	377358.364839	52.022170
3319.431068	377017.880906	52.027175
3319.102209	376680.043219	52.032180
3317.794372	376351.641699	52.037185
3317.468606	375998.383456	52.042189
3316.819927	375655.958298	52.047194
3316.044065	375326.752053	52.052199
3315.570719	374982.233079	52.057204
3314.541607	374648.075721	52.062209
3314.084737	374308.941134	52.067213
3313.553044	373979.532752	52.072218
3312.782982	373636.524736	52.077223
3312.299409	373290.466863	52.082228
3311.275105	372950.342415	52.087233
3310.884072	372611.336071	52.092237
3310.123275	372286.554796	52.097242
3309.596967	371942.705622	52.102247
3309.093419	371595.975409	52.107252
3308.056721	371257.619873	52.112257
3307.487544	370923.130808	52.117261
3306.875819	370582.336783	52.122266
3305.828582	370249.240878	52.127271
3305.366297	369917.754345	52.132276
3305.009286	369577.802414	52.137281
3304.359376	369241.175943	52.142285
3303.394892	368905.334377	52.147290
3302.816589	368561.338917	52.152295
3302.156226	368215.929010	52.157300
3301.335384	367885.552118	52.162305
3300.425070	367543.509233	52.167309
3300.010189	367214.182500	52.172314
3298.884424	366877.587591	52.177319
3298.384596	366544.910972	52.182324
3297.706416	366224.650449	52.187329
3297.027410	365888.587995	52.192333
3296.326567	365553.391518	52.197338
3295.506642	365218.542128	52.202343
3295.130162	364898.682378	52.207348
3294.347646	364569.725035	52.212353
3294.033285	364235.373595	52.217357
3293.350626	363911.840580	52.222362
3292.465306	363580.068110	52.227367
3292.172238	363243.797769	52.232372
3291.208995	362918.266609	52.237377
3290.750132	362576.038257	52.242381
3289.570747	362246.287360	52.247386
3288.893317	361915.513284	52.252391
3288.459392	361577.853692	52.257396
3287.654715	361255.390100	52.262401
3286.893967	360930.194717	52.267405
3286.635160	360591.966012	52.272410
3285.896335	360265.159539	52.277415
3285.136096	359938.583222	52.282420
3284.481346	359608.247444	52.287425
3283.558027	359269.096637	52.292429
3283.113165	358950.581019	52.297434
3282.239208	358618.797251	52.302439
3281.798289	358293.686072	52.307444
3280.610619	357964.644803	52.312449
3280.188352	357641.612972	52.317453
3279.473541	357319.566833	52.322458
3278.924909	356992.148383	52.327463
3278.128733	356671.459597	52.332468
3277.192313	356353.513820	52.337473
3277.018252	356027.200364	52.342477
3276.159418	355704.810283	52.347482
3275.500070	355377.118832	52.352487
3275.011465	355040.287775	52.357492
3274.012059	354730.637842	52.362497
3273.075879	354407.335594	52.367501
3272.997751	354077.838786	52.372506
3272.136214	353757.701727	52.377511
3271.239577	353437.059252	52.382516
3270.931991	353121.029725	52.387521
3270.500395	352789.468331	52.392525
3269.355249	352471.378698	52.397530
3268.593591	352152.844733	52.402535
3268.462851	351828.533734	52.407540
3267.689407	351507.020105	52.412545
3266.954155	351177.558043	52.417549
3266.486838	350843.928617	52.422554
3265.391676	350513.348676	52.427559
3265.001421	350188.687001	52.432564
3264.256723	349869.780411	52.437569
3263.773289	349541.642841	52.442573
3262.954417	349215.108869	52.447578
3261.840265	348899.461875	52.452583
3261.603545	348568.352557	52.457588
3260.364549	348253.637859	52.462593
3259.903501	347930.781049	52.467597
3259.214853	347612.921471	52.472602
3258.472160	347304.943993	52.477607
3257.972557	346980.509777	52.482612
3257.187138	346667.165177	52.487617
3256.642323	346344.287051	52.492621
3256.086203	346032.226202	52.497626
3255.159061	345714.444586	52.502631
3254.710989	345385.869804	52.507636
3253.838052	345067.465176	52.512641
3252.990216	344747.044035	52.517645
3252.599036	344441.566298	52.522650
3251.984580	344128.868079	52.527655
3251.398730	343816.418205	52.532660
3250.365425	343501.644816	52.537665
3249.821891	343176.890771	52.542669
3249.194256	342866.504258	52.547674
3248.436790	342550.078613	52.552679
3247.969383	342229.380030	52.557684
3247.131281	341909.451103	52.562689
3246.355110	341599.285195	52.567693
3245.793104	341286.767467	52.572698
3244.976508	340982.917556	52.577703
3244.462853	340664.738075	52.582708
3243.542191	340347.410442	52.587713
3243.207814	340036.784954	52.592717
3242.413923	339726.357884	52.597722
3241.457768	339411.678452	52.602727
3240.943717	339097.920278	52.607732
3240.188387	338797.308338	52.612737
3240.151861	338476.904021	52.617741
3239.194301	338161.862239	52.622746
3238.637192	337855.257854	52.627751
3238.122757	337529.476843	52.632756
3237.259088	337217.470333	52.637761
3236.539994	336897.369809	52.642765
3235.809492	336588.877665	52.647770
3235.015510	336281.208730	52.652775
3234.658806	335964.050223	52.657780
3234.054413	335653.344501	52.662785
3232.948636	335343.811298	52.667789
3232.121852	335032.195975	52.672794
3231.420407	334716.358959	52.677799
3231.095143	334405.272391	52.682804
3230.601225	334095.840360	52.687809
3229.984464	333784.338854	52.692813
3229.339368	333471.567544	52.697818
3228.278636	333158.911491	52.702823
3227.951560	332843.643110	52.707828
3226.839760	332530.075844	52.712833
3226.271020	332217.846929	52.717837
3225.788788	331905.908453	52.722842
3224.823335	331600.511461	52.727847
3224.206315	331290.093661	52.732852
3223.501653	330984.907383	52.737857
3223.001805	330671.897085	52.742861
3222.489649	330363.648171	52.747866
3221.529036	330061.069847	52.752871
3220.885954	329752.915461	52.757876
3220.097709	329443.688020	52.762881
3219.560903	329131.135290	52.767885
3219.015493	328829.097288	52.772890
3217.998398	328529.424036	52.777895
3217.835610	328214.109646	52.782900
3216.643843	327922.099469	52.787905
3216.071045	327616.751243	52.792909
3215.608104	327295.879438	52.797914
3214.375719	327006.723714	52.802919
3214.110939	326698.828082	52.807924
3213.700524	326401.316522	52.812929
3213.102330	326082.065120	52.817933
3212.210737	325783.659876	52.822938
3211.309707	325486.935392	52.827943
3210.820927	325168.630525	52.832948
3210.218256	324871.347366	52.837953
3209.865860	324565.519678	52.842957
3209.045934	324245.710489	52.847962
3208.011982	323945.844282	52.852967
3207.483372	323641.823299	52.857972
3206.600618	323334.521841	52.862977
3206.181601	323033.052870	52.867981
3205.394158	322727.847390	52.872986
3204.579541	322433.517081	52.877991
3204.280783	322126.017004	52.882996
3203.380591	321824.976343	52.888001
3202.676251	321524.591113	52.893005
3201.972940	321223.288066	52.898010
3201.142504	320931.501317	52.903015
3200.607224	320621.232562	52.908020
3200.224744	320333.905179	52.913025
3199.435263	320024.285647	52.918029
3198.507919	319725.304543	52.923034
3197.766234	319433.575254	52.928039
3197.376437	319127.046731	52.933044
3196.661670	318831.797479	52.938049
3195.845239	318530.223231	52.943053
3195.466437	318233.569417	52.948058
3194.683351	317933.261091	52.953063
3194.154203	317635.228735	52.958068
3193.477009	317341.802156	52.963073
3192.862201	317041.617167	52.968077
3192.087810	316737.637059	52.973082
3191.052291	316432.831572	52.978087
3190.639062	316135.973001	52.983092
3190.076468	315832.465833	52.988097
3189.082022	315546.901214	52.993101
3188.678496	315233.461875	52.998106
3187.884520	314945.317502	53.003111
3187.315076	314645.270838	53.008116
3186.487021	314348.803633	53.013121
3186.063984	314042.849979	53.018125
3185.530738	313749.211793	53.023130
3184.612640	313462.305160	53.028135
3184.189585	313137.454793	53.033140
3182.960119	312851.385141	53.038145
3182.332865	312555.645015	53.043149
3181.747070	312262.749485	53.048154
3181.269660	311971.669429	53.053159
3180.619404	311675.446730	53.058164
3179.676108	311381.332198	53.063169
3178.930418	311089.579264	53.068173
3178.539217	310791.632585	53.073178
3177.918497	310504.976693	53.078183
3177.319034	310200.007776	53.083188
3176.574283	309916.960524	53.088193
3175.896947	309617.630047	53.093197
3175.214333	309321.253537	53.098202
3174.816199	309021.215285	53.103207
3174.146047	308724.275085	53.108212
3173.406637	308426.861277	53.113217
3172.544190	308128.396679	53.118221
3172.245367	307840.766644	53.123226
3171.350934	307544.699391	53.128231
3170.817823	307238.999395	53.133236
3170.200871	306950.500890	53.138241
3169.138784	306642.107438	53.143245
3168.507997	306353.125928	53.148250
3167.843296	306061.882723	53.153255
3167.264208	305759.598813	53.158260
3166.396304	305472.639164	53.163265
3165.568200	305177.778295	53.168269
3164.987637	304879.643487	53.173274
3164.299293	304595.225568	53.178279
3164.013945	304297.959536	53.183284
3162.871900	304016.133300	53.188289
3162.539765	303718.440511	53.193293
3162.073805	303427.847761	53.198298
3160.899522	303142.510593	53.203303
3160.607581	302852.729512	53.208308
3159.871458	302559.962215	53.213313
3159.326215	302262.019997	53.218317
3158.414546	301977.097384	53.223322
3157.553484	301682.412699	53.228327
3157.170208	301389.027015	53.233332
3156.372197	301103.600916	53.238337
3155.586873	300815.370993	53.243341
3154.932274	300520.320351	53.248346
3154.371605	300238.853329	53.253351
3153.905501	299944.128321	53.258356
3153.159403	299662.766028	53.263361
3152.227795	299372.162802	53.268365
3151.602993	299081.230389	53.273370
3150.761677	298797.742502	53.278375
3150.535955	298501.729026	53.283380
3149.829849	298216.614381	53.288385
3149.155984	297921.154684	53.293389
3148.651382	297644.411233	53.298394
3147.616986	297357.513531	53.303399
3147.078103	297060.146504	53.308404
3146.380661	296773.933101	53.313409
3145.800925	296488.617439	53.318413
3144.868828	296194.443665	53.323418
3144.188594	295911.842528	53.328423
3143.767267	295623.826467	53.333428
3143.255409	295330.985565	53.338433
3142.254319	295042.933052	53.343437
3141.633783	294755.736728	53.348442
3141.067774	294467.971092	53.353447
3140.572280	294180.652306	53.358452
3139.814591	293891.133497	53.363457
3138.984454	293606.006128	53.368461
3138.632941	293322.687229	53.373466
3137.715994	293039.737574	53.378471
3137.149187	292747.538434	53.383476
3136.259815	292458.165904	53.388481
3135.416462	292170.390176	53.393485
3134.691723	291889.064060	53.398490
3134.016422	291613.612780	53.403495
3133.671112	291327.871024	53.408500
3132.949858	291051.382210	53.413505
3132.356215	290760.763856	53.418509
3131.947233	290461.074946	53.423514
3130.989271	290185.463075	53.428519
3130.284289	289907.697069	53.433524
3129.688743	289629.455040	53.438529
3128.850888	289342.897657	53.443533
3128.225955	289057.452336	53.448538
3127.614615	288772.870481	53.453543
3127.322081	288481.667208	53.458548
3126.277231	288200.209529	53.463553
3125.182608	287922.248558	53.468557
3124.725446	287628.727470	53.473562
3123.807112	287360.059341	53.478567
3123.418918	287082.571606	53.483572
3123.085765	286803.088428	53.488577
3122.435046	286523.960885	53.493581
3121.551645	286239.623532	53.498586
3120.622203	285963.850482	53.503591
3120.169369	285672.644591	53.508596
3119.326014	285397.697937	53.513601
3118.636414	285122.624881	53.518605
3118.291042	284845.281439	53.523610
3117.448918	284562.184220	53.528615
3116.577833	284284.490627	53.533620
3116.020720	284009.981621	53.538625
3115.462253	283717.339344	53.543629
3114.768831	283445.576648	53.548634
3114.004680	283171.201765	53.553639
3113.442874	282893.101820	53.558644
3112.801931	282620.082412	53.563649
3112.249424	282339.892298	53.568653
3111.695847	282066.374879	53.573658
3110.963778	281788.224884	53.578663
3110.141394	281510.012641	53.583668
3109.444059	281227.832899	53.588673
3109.012871	280953.760759	53.593677
3108.242706	280673.426012	53.598682
3107.361593	280395.273511	53.603687
3107.137486	280104.613870	53.608692
3106.484643	279834.549420	53.613697
3105.427762	279550.821392	53.618701
3104.800169	279269.011863	53.623706
3103.910084	278995.037094	53.628711
3103.670387	278717.291881	53.633716
3102.869927	278443.175432	53.638721
3101.762474	278160.422785	53.643725
3101.529078	277877.557220	53.648730
3100.523537	277612.641639	53.653735
3100.063509	277328.079972	53.658740
3099.458874	277056.962969	53.663745
3098.503584	276787.225769	53.668749
3098.156881	276510.770444	53.673754
3097.124215	276241.580254	53.678759
3096.698920	275967.505862	53.683764
3095.782227	275692.948905	53.688769
3095.356471	275424.630399	53.693773
3094.692832	275148.963691	53.698778
3094.149636	274878.804555	53.703783
3093.504279	274608.254087	53.708788
3092.673165	274335.288051	53.713793
3091.992618	274063.189587	53.718797
3091.541618	273783.312417	53.723802
3090.657489	273510.584019	53.728807
3090.141096	273232.652833	53.733812
3089.566694	272971.336240	53.738817
3089.088725	272688.814721	53.743821
3088.067719	272398.942412	53.748826
3087.448757	272119.372153	53.753831
3086.911658	271836.885592	53.758836
3086.100162	271559.510715	53.763841
3085.469899	271297.082610	53.768845
3085.074289	271017.859250	53.773850
3084.136625	270739.282047	53.778855
3083.478322	270464.480959	53.783860
3082.758726	270196.769843	53.788865
3081.893141	269918.767239	53.793869
3081.363108	269638.241194	53.798874
3080.407219	269384.804513	53.803879
3079.793313	269098.281413	53.808884
3079.008997	268835.318089	53.813889
3078.505563	268564.975549	53.818893
3077.990607	268300.110617	53.823898
3076.995282	268038.352540	53.828903
3076.425672	267763.589333	53.833908
3075.654680	267501.923326	53.838913
3075.052580	267228.464393	53.843917
3074.638186	266967.684524	53.848922
3073.676975	266701.592066	53.853927
3073.230964	266432.591241	53.858932
3072.717861	266163.703053	53.863937
3071.553551	265898.203468	53.868941
3071.127249	265632.154276	53.873946
3070.589451	265372.948344	53.878951
3069.826340	265104.456895	53.883956
3068.972915	264832.796396	53.888961
3068.253751	264576.573949	53.893965
3067.962078	264310.911760	53.898970
3067.262767	264047.326240	53.903975
3066.428854	263777.038645	53.908980
3065.789050	263502.772982	53.913985
3065.281937	263254.514808	53.918989
3064.777919	262977.604849	53.923994
3063.980683	262700.970728	53.928999
3063.272944	262439.476083	53.934004
3062.781894	262178.252962	53.939009
3061.977119	261903.607190	53.944013
3061.432340	261639.922622	53.949018
3060.485129	261380.555097	53.954023
3060.114396	261103.549224	53.959028
3059.272866	260841.109294	53.964033
3058.594292	260570.163037	53.969037
3057.625431	260302.013493	53.974042
3056.958059	260041.227595	53.979047
3056.455565	259772.801001	53.984052
3055.906444	259518.898626	53.989057
3055.105395	259253.193902	53.994061
3054.416689	258990.706054	53.999066
3053.893594	258727.657438	54.004071
3053.065784	258467.840766	54.009076
3052.724560	258200.408954	54.014081
3052.121922	257939.971438	54.019085
3051.280244	257671.549772	54.024090
3050.540286	257411.083622	54.029095
3049.668857	257141.724964	54.034100
3049.319149	256885.909106	54.039105
3048.295458	256618.357874	54.044109
3048.104692	256351.897561	54.049114
3047.002518	256101.753566	54.054119
3046.173088	255840.692154	54.059124
3045.505613	255571.354029	54.064129
3045.279449	255316.921126	54.069133
3044.770994	255058.254719	54.074138
3043.831817	254799.554936	54.079143
3043.270699	254524.216537	54.084148
3042.653102	254273.921609	54.089153
3041.807943	254004.588178	54.094157
3041.098153	253736.354237	54.099162
3039.996649	253480.890695	54.104167
3039.608694	253221.290773	54.109172
3039.203433	252960.802601	54.114177
3038.702347	252708.046424	54.119181
3038.044322	252439.602379	54.124186
3037.005911	252189.478642	54.129191
3036.450438	251906.910528	54.134196
3036.057763	251656.379722	54.139201
3035.061546	251394.688511	54.144205
3034.553535	251132.283751	54.149210
3033.902268	250870.666060	54.154215
3033.353212	250610.560585	54.159220
3032.479313	250356.517031	54.164225
3031.597650	250094.071139	54.169229
3031.331279	249825.594585	54.174234
3030.254010	249580.854202	54.179239
3029.539439	249314.945136	54.184244
3029.250807	249066.337143	54.189249
3028.166405	248812.889562	54.194253
3027.798803	248543.972769	54.199258
3027.044528	248296.636604	54.204263
3026.377805	248030.773057	54.209268
3026.113139	247776.764487	54.214273
3025.199759	247523.368343	54.219277
3024.666945	247253.232121	54.224282
3023.725646	247004.959950	54.229287
3023.514674	246742.744577	54.234292
3022.621981	246485.781694	54.239297
3021.735855	246223.292132	54.244301
3021.458028	245960.248380	54.249306
3020.400238	245701.275767	54.254311
3019.672660	245446.987988	54.259316
3018.937561	245182.668381	54.264321
3018.362589	244929.808935	54.269325
3017.759667	244670.129599	54.274330
3017.010187	244418.164551	54.279335
3016.609642	244158.887074	54.284340
3016.106060	243905.687185	54.289345
3015.198767	243658.332326	54.294349
3014.348727	243392.328232	54.299354
3013.616163	243135.575452	54.304359
3013.075324	242872.655709	54.309364
3012.592163	242625.108352	54.314369
3011.663873	242368.006109	54.319373
3011.560203	242106.546654	54.324378
3010.221865	241850.427116	54.329383
3009.792530	241602.669526	54.334388
3009.354580	241354.098919	54.339393
3008.099423	241089.869940	54.344397
3007.823377	240838.702800	54.349402
3006.863101	240587.262516	54.354407
3006.295232	240330.056547	54.359412
3005.943516	240073.147959	54.364417
3004.969869	239817.407889	54.369421
3004.550782	239571.180735	54.374426
3003.882438	239310.529716	54.379431
3003.085629	239059.830755	54.384436
3002.441823	238812.443958	54.389441
3001.631566	238548.099334	54.394445
3001.371187	238299.074172	54.399450
3000.504991	238041.334838	54.404455
2999.647225	237791.004836	54.409460
2999.012605	237539.188623	54.414465
2998.200719	237288.699713	54.419469
2998.147394	237027.905706	54.424474
2996.863493	236791.039499	54.429479
2996.408980	236526.057729	54.434484
2995.571808	236269.158287	54.439489
2994.988406	236027.395688	54.444493
2994.634297	235765.990304	54.449498
2993.947996	235520.043649	54.454503
2992.920456	235266.079640	54.459508
2992.453464	235016.254461	54.464513
2991.475359	234770.610409	54.469517
2991.114103	234517.535847	54.474522
2990.425722	234272.254546	54.479527
2989.848856	234012.442132	54.484532
2989.110554	233760.243975	54.489537
2988.023452	233513.397998	54.494541
2987.621467	233258.397856	54.499546
2986.758804	233013.758346	54.504551
2986.087772	232768.707168	54.509556
2985.473281	232522.450899	54.514561
2984.882206	232279.170698	54.519565
2984.377119	232027.882198	54.524570
2983.539349	231782.121496	54.529575
2983.097932	231536.476922	54.534580
2982.296323	231281.952654	54.539585
2981.754741	231035.561363	54.544589
2980.915050	230788.963287	54.549594
2980.133820	230547.703701	54.554599
2979.832057	230290.276689	54.559604
2979.089145	230045.804102	54.564609
2978.265240	229800.530202	54.569613
2977.632006	229549.345042	54.574618
2976.865301	229306.915171	54.579623
2976.251392	229051.043331	54.584628
2976.019078	228808.784827	54.589633
2974.841251	228566.625736	54.594637
2974.466413	228318.483997	54.599642
2973.889549	228071.418865	54.604647
2973.190220	227812.024958	54.609652
2972.365867	227568.132199	54.614657
2971.547078	227324.010092	54.619661
2970.975129	227070.785361	54.624666
2970.116425	226838.001251	54.629671
2969.516063	226584.986144	54.634676
2968.841863	226336.719249	54.639681
2968.287912	226106.664160	54.644685
2967.650551	225849.226889	54.649690
2966.597240	225612.008562	54.654695
2966.237334	225360.830446	54.659700
2965.825847	225131.723001	54.664705
2964.698236	224882.335555	54.669709
2964.524210	224645.082646	54.674714
2963.567176	224409.494746	54.679719
2963.142120	224146.771579	54.684724
2962.538014	223886.890980	54.689729
2961.706898	223660.934808	54.694733
2960.817880	223408.662571	54.699738
2960.163773	223169.109473	54.704743
2959.436150	222918.073520	54.709748
2958.748193	222686.343481	54.714753
2957.735098	222457.007910	54.719757
2957.523875	222208.718520	54.724762
2956.667583	221974.967721	54.729767
2955.992041	221738.948562	54.734772
2955.495921	221493.214343	54.739777
2954.435217	221261.076564	54.744781
2954.184262	221021.962705	54.749786
2953.325130	220783.735121	54.754791
2953.298411	220542.614171	54.759796
2952.492439	220304.506976	54.764801
2951.429195	220065.550197	54.769805
2950.958606	219816.456768	54.774810
2950.265751	219577.111948	54.779815
2949.492518	219338.582579	54.784820
2949.277352	219095.675826	54.789825
2948.317436	218854.580784	54.794829
2947.823473	218610.052232	54.799834
2947.160376	218365.347608	54.804839
2946.362601	218121.823491	54.809844
2945.761427	217879.083737	54.814849
2944.888419	217639.302811	54.819853
2944.914827	217396.465331	54.824858
2943.955364	217154.115714	54.829863
2943.296390	216906.984162	54.834868
2942.714610	216651.898381	54.839873
2941.856350	216409.344361	54.844877
2941.365978	216161.946881	54.849882
2940.595670	215916.567565	54.854887
2939.768149	215675.347755	54.859892
2939.400292	215425.680504	54.864897
2938.228349	215192.217796	54.869901
2938.045704	214934.109340	54.874906
2937.018574	214707.435182	54.879911
2936.139033	214466.953385	54.884916
2935.953191	214214.957867	54.889921
2935.105125	213974.052796	54.894925
2934.452932	213724.296784	54.899930
2933.619048	213497.201512	54.904935
2932.991163	213256.620556	54.909940
2932.374211	213010.820143	54.914945
2931.459249	212778.076081	54.919949
2930.970132	212538.939507	54.924954
2930.362079	212298.575276	54.929959
2929.598351	212050.281515	54.934964
2929.249954	211812.143563	54.939969
2928.245125	211578.896142	54.944973
2927.813311	211332.970892	54.949978
2926.820246	211107.118255	54.954983
2926.061720	210857.911835	54.959988
2925.587461	210630.324115	54.964993
2924.415066	210392.729166	54.969997
2924.027049	210156.067317	54.975002
2923.450529	209931.616582	54.980007
2922.662984	209697.437966	54.985012
2922.418138	209471.905417	54.990017
2921.342999	209235.674009	54.995021
2921.208536	208985.268872	55.000026
2920.497393	208754.416293	55.005031
2919.563922	208507.665089	55.010036
2918.940212	208268.451318	55.015041
2918.132172	208040.811311	55.020045
2917.428046	207798.099374	55.025050
2917.007813	207573.759694	55.030055
2915.934596	207332.177135	55.035060
2916.093681	207088.045916	55.040065
2915.156572	206864.503414	55.045069
2914.508998	206619.916364	55.050074
2913.360904	206382.218473	55.055079
2912.745231	206157.342292	55.060084
2912.088687	205916.921232	55.065089
2911.244307	205683.950603	55.070093
2910.688413	205451.037029	55.075098
2910.051929	205224.335033	55.080103
2909.113478	204990.936603	55.085108
2908.530442	204773.340160	55.090113
2907.955847	204544.849270	55.095117
2907.552886	204304.483738	55.100122
2906.991319	204079.568758	55.105127
2906.177187	203849.960426	55.110132
2905.619567	203608.998679	55.115137
2904.793164	203384.141072	55.120141
2904.287364	203150.337946	55.125146
2903.539893	202916.128627	55.130151
2902.705182	202684.988357	55.135156
2902.125779	202448.718174	55.140161
2901.334154	202232.933305	55.145165
2901.173909	201995.211513	55.150170
2900.181629	201764.761713	55.155175
2899.856879	201533.176370	55.160180
2898.858945	201301.864014	55.165185
2898.198319	201077.841978	55.170189
2897.693691	200830.978945	55.175194
2896.929362	200604.748244	55.180199
2896.662022	200371.224362	55.185204
2895.665559	200140.247501	55.190209
2894.546363	199893.702318	55.195213
2894.185590	199671.381922	55.200218
2893.661759	199436.642824	55.205223
2892.732283	199216.946688	55.210228
2892.235638	198985.742883	55.215233
2891.525123	198756.762671	55.220237
2890.961575	198526.169517	55.225242
2890.449821	198292.680553	55.230247
2889.748718	198061.424026	55.235252
2888.906282	197825.151781	55.240257
2887.665472	197601.121443	55.245261
2887.452677	197367.500126	55.250266
2886.773063	197155.356942	55.255271
2885.967236	196924.109240	55.260276
2885.616914	196692.306890	55.265281
2884.874005	196470.912892	55.270285
2884.224169	196241.386787	55.275290
2883.546833	196018.266505	55.280295
2882.680405	195786.931642	55.285300
2882.061169	195560.813871	55.290305
2881.090638	195344.906788	55.295309
2880.710922	195112.327237	55.300314
2879.813072	194902.187359	55.305319
2879.192645	194676.010050	55.310324
2878.735214	194444.692814	55.315329
2878.102264	194219.868276	55.320333
2877.368458	193996.727558	55.325338
2876.667817	193772.462860	55.330343
2875.902073	193546.720765	55.335348
2875.593971	193324.686213	55.340353
2874.466568	193107.261171	55.345357
2874.424031	192878.951861	55.350362
2873.696825	192665.371573	55.355367
2872.832571	192430.234560	55.360372
2872.433544	192205.560139	55.365377
2871.923653	191982.621974	55.370381
2871.222075	191746.609972	55.375386
2870.429564	191516.148194	55.380391
2869.716743	191282.074165	55.385396
2869.359395	191051.571110	55.390401
2868.302694	190838.572574	55.395405
2867.754325	190598.406792	55.400410
2866.849469	190372.599448	55.405415
2866.642167	190138.934347	55.410420
2866.044286	189910.205139	55.415425
2864.956138	189675.638482	55.420429
2864.470591	189453.026123	55.425434
2863.795533	189227.912966	55.430439
2863.140394	189001.589052	55.435444
2862.677602	188763.403637	55.440449
2861.627899	188536.750014	55.445453
2861.269883	188304.161000	55.450458
2860.777237	188070.296754	55.455463
2859.920982	187848.386746	55.460468
2859.306332	187605.460295	55.465473
2858.566199	187387.070906	55.470477
2857.973153	187149.830283	55.475482
2857.050792	186931.153829	55.480487
2856.272162	186701.858093	55.485492
2855.988205	186467.905206	55.490497
2854.978699	186243.406361	55.495501
2854.308019	186006.718206	55.500506
2853.790610	185790.909067	55.505511
2853.121707	185559.095423	55.510516
2852.631940	185324.710231	55.515521
2851.776570	185095.892636	55.520525
2851.249513	184878.982542	55.525530
2850.213294	184655.360791	55.530535
2849.941129	184426.237946	55.535540
2849.428699	184193.477813	55.540545
2848.464624	183966.972996	55.545549
2848.063818	183738.230218	55.550554
2847.073175	183502.890634	55.555559
2846.308273	183272.426919	55.560564
2845.815391	183052.886924	55.565569
2845.034994	182823.878191	55.570573
2844.679339	182597.258527	55.575578
2843.722559	182369.208706	55.580583
2843.085271	182144.366009	55.585588
2843.072827	181910.826246	55.590593
2841.862047	181691.177724	55.595597
2841.412662	181454.872858	55.600602
2840.691439	181217.467463	55.605607
2839.624861	180995.929670	55.610612
2839.214283	180767.572712	55.615617
2838.263514	180538.043183	55.620621
2837.634191	180311.885733	55.625626
2836.981479	180092.843799	55.630631
2836.370873	179871.074187	55.635636
2836.110394	179645.090785	55.640641
2834.880490	179413.614389	55.645645
2834.346648	179188.236371	55.650650
2833.667695	178974.991900	55.655655
2832.696658	178747.917376	55.660660
2832.433819	178525.527273	55.665665
2831.605163	178311.877364	55.670669
2830.951414	178076.208526	55.675674
2830.155069	177860.202646	55.680679
2829.653459	177640.793240	55.685684
2829.320796	177419.717412	55.690689
2828.506474	177195.717251	55.695693
2827.912634	176976.949176	55.700698
2827.059097	176750.693572	55.705703
2826.523261	176527.772188	55.710708
2825.607695	176304.873982	55.715713
2824.892268	176094.104701	55.720717
2824.583072	175858.902567	55.725722
2823.685904	175652.844909	55.730727
2823.112458	175439.728921	55.735732
2822.795491	175195.539572	55.740737
2821.634603	174967.981502	55.745741
2820.943982	174746.734981	55.750746
2820.300840	174534.753983	55.755751
2819.251008	174318.984790	55.760756
2819.085774	174102.987617	55.765761
2817.985172	173889.886902	55.770765
2817.773742	173651.362495	55.775770
2817.185471	173437.470802	55.780775
2816.557563	173214.404007	55.785780
2815.747856	172989.853790	55.790785
2815.124221	172782.355669	55.795789
2814.577496	172556.519865	55.800794
2813.793823	172338.493494	55.805799
2812.762812	172123.254538	55.810804
2812.340489	171897.771584	55.815809
2811.394030	171682.839569	55.820813
2810.911127	171461.667267	55.825818
2810.054518	171254.748160	55.830823
2809.549412	171039.533548	55.835828
2809.282980	170813.892200	55.840833
2808.014706	170595.685128	55.845837
2807.864029	170386.624018	55.850842
2807.144202	170165.712728	55.855847
2806.837889	169939.459597	55.860852
2806.188586	169719.328130	55.865857
2805.079433	169501.127420	55.870861
2804.578532	169277.693978	55.875866
2804.124637	169061.083316	55.880871
2803.138241	168834.397525	55.885876
2802.450806	168604.105051	55.890881
2801.494654	168387.628593	55.895885
2801.061863	168176.195229	55.900890
2800.327580	167964.670903	55.905895
2800.061342	167745.075010	55.910900
2799.392700	167525.989187	55.915905
2798.556261	167305.011050	55.920909
2797.841611	167078.241772	55.925914
2797.295203	166864.659223	55.930919
2796.554801	166646.085779	55.935924
2795.935916	166414.574957	55.940929
2795.235322	166207.442101	55.945933
2794.457043	165993.418013	55.950938
2794.002261	165771.930642	55.955943
2793.345236	165552.294953	55.960948
2792.699522	165326.224685	55.965953
2791.826946	165111.622951	55.970957
2791.205265	164886.912103	55.975962
2790.660912	164669.641560	55.980967
2790.010906	164450.100277	55.985972
2789.342850	164225.820389	55.990977
2788.779218	164004.424373	55.995981
2788.118637	163777.641152	56.000986
2787.634094	163587.450552	56.005991
2786.913826	163278.693813	56.010996
2786.576513	163052.957352	56.016001
2785.613851	162841.523667	56.021005
2784.885638	162614.046348	56.026010
2784.563607	162383.416481	56.031015
2783.472979	162162.649105	56.036020
2783.132507	161934.796769	56.041025
2782.272534	161716.322320	56.046029
2781.396755	161487.197166	56.051034
2780.825077	161267.993204	56.056039
2779.846126	161054.258575	56.061044
2779.755111	160814.676862	56.066049
2778.602890	160602.358201	56.071053
2778.351000	160387.558851	56.076058
2777.563009	160158.237589	56.081063
2776.412167	159945.121661	56.086068
2776.328393	159721.006001	56.091073
2775.288802	159504.200870	56.096077
2774.883168	159269.421542	56.101082
2774.043949	159048.544595	56.106087
2773.710510	158839.666547	56.111092
2772.852043	158617.765577	56.116097
2771.945263	158396.089786	56.121101
2771.207101	158173.765751	56.126106
2770.913560	157950.381093	56.131111
2769.989212	157740.878556	56.136116
2769.627598	157519.973739	56.141121
2769.059814	157298.747026	56.146125
2768.368916	157074.680878	56.151130
2767.473570	156850.839253	56.156135
2766.800751	156635.887997	56.161140
2766.275794	156400.129876	56.166145
2765.384526	156190.898441	56.171149
2764.986450	155968.013483	56.176154
2764.114509	155746.501673	56.181159
2763.150263	155531.476366	56.186164
2762.637154	155299.817221	56.191169
2761.938461	155091.400997	56.196173
2761.453388	154873.265791	56.201178
2760.931169	154654.794653	56.206183
2760.001931	154437.101246	56.211188
2759.638120	154215.811278	56.216193
2758.444999	154001.607315	56.221197
2757.575304	153787.467886	56.226202
2757.385250	153580.365940	56.231207
2756.632821	153366.604666	56.236212
2756.173359	153144.307276	56.241217
2755.358413	152928.397798	56.246221
2754.999224	152709.570254	56.251226
2754.000307	152500.645611	56.256231
2753.135834	152284.938807	56.261236
2752.553631	152054.876361	56.266241
2751.918617	151850.105428	56.271245
2751.197383	151629.397604	56.276250
2750.722990	151424.730964	56.281255
2750.176938	151219.810025	56.286260
2749.624544	150993.677765	56.291265
2748.914151	150784.247969	56.296269
2748.268172	150559.010533	56.301274
2747.490675	150344.954951	56.306279
2746.795571	150119.931676	56.311284
2746.381297	149900.953526	56.316289
2745.295561	149691.590179	56.321293
2744.724178	149475.397814	56.326298
2744.439127	149258.792948	56.331303
2743.433305	149045.379427	56.336308
2743.045204	148824.510650	56.341313
2742.234048	148611.819014	56.346317
2741.878584	148386.169317	56.351322
2741.088645	148167.135291	56.356327
2740.197408	147951.880718	56.361332
2739.707977	147725.418072	56.366337
2738.894958	147519.990838	56.371341
2738.260232	147304.217040	56.376346
2737.599395	147082.094422	56.381351
2736.960976	146868.154227	56.386356
2736.271652	146646.433130	56.391361
2735.438251	146439.846888	56.396365
2735.275838	146213.597345	56.401370
2734.578504	145996.482529	56.406375
2733.722241	145783.041663	56.411380
2733.234390	145549.833437	56.416385
2732.317381	145339.760163	56.421389
2731.483956	145119.419664	56.426394
2731.017550	144905.313006	56.431399
2730.331280	144682.169226	56.436404
2729.846438	144468.958021	56.441409
2728.909241	144254.295008	56.446413
2728.502657	144031.962980	56.451418
2727.943142	143822.465934	56.456423
2726.724642	143605.717095	56.461428
2726.301027	143380.901766	56.466433
2725.519257	143176.082469	56.471437
2724.880414	142958.496605	56.476442
2723.932517	142739.982790	56.481447
2723.213931	142530.024115	56.486452
2722.870625	142309.968977	56.491457
2721.599571	142116.327350	56.496461
2721.179347	141893.326697	56.501466
2720.744492	141693.125677	56.506471
2720.173864	141479.148166	56.511476
2719.376863	141260.366856	56.516481
2718.939360	141053.499562	56.521485
2717.989095	140831.734202	56.526490
2717.507705	140627.850024	56.531495
2716.593386	140410.757924	56.536500
2716.008388	140204.123080	56.541505
2715.427598	140001.808996	56.546509
2714.909495	139779.360290	56.551514
2714.284229	139577.780327	56.556519
2713.381178	139367.555050	56.561524
2712.911211	139152.688628	56.566529
2712.533228	138943.729926	56.571533
2711.921437	138724.899518	56.576538
2710.830618	138514.316104	56.581543
2710.352566	138300.397273	56.586548
2709.620997	138078.808134	56.591553
2709.331875	137880.502384	56.596557
2708.592319	137669.767654	56.601562
2708.010710	137444.233664	56.606567
2706.908767	137222.264924	56.611572
2706.231660	137006.862376	56.616577
2705.555467	136800.773698	56.621581
2704.863205	136590.737915	56.626586
2704.306149	136373.313669	56.631591
2703.346333	136168.100139	56.636596
2703.070544	135941.449327	56.641601
2702.235512	135748.414994	56.646605
2701.372710	135535.212348	56.651610
2700.900980	135320.589982	56.656615
2699.961619	135122.786934	56.661620
2699.390420	134902.936717	56.666625
2698.648185	134705.168797	56.671629
2698.317859	134503.322638	56.676634
2697.343740	134288.419078	56.681639
2696.682030	134083.109485	56.686644
2696.468840	133868.545812	56.691649
2695.096548	133672.167801	56.696653
2694.833633	133468.184050	56.701658
2694.355154	133243.085371	56.706663
2693.496427	133056.500443	56.711668
2693.137969	132838.829835	56.716673
2692.341821	132631.011333	56.721677
2691.798046	132419.978696	56.726682
2691.001382	132204.783137	56.731687
2689.999807	132003.911934	56.736692
2689.939686	131796.389378	56.741697
2689.001158	131593.694643	56.746701
2688.185159	131376.387132	56.751706
2687.692143	131161.418107	56.756711
2686.980669	130959.924033	56.761716
2686.203649	130740.798840	56.766721
2685.645146	130540.185359	56.771725
2685.270152	130326.867921	56.776730
2684.690859	130113.749588	56.781735
2683.603641	129918.863820	56.786740
2682.961348	129691.812397	56.791745
2682.210510	129497.193802	56.796749
2681.615439	129287.259584	56.801754
2681.163742	129070.725034	56.806759
2680.507548	128869.160996	56.811764
2679.652175	128653.138182	56.816769
2678.910339	128450.574667	56.821773
2678.287950	128241.821133	56.826778
2678.052621	128041.390287	56.831783
2677.135773	127834.921787	56.836788
2676.952352	127614.317298	56.841793
2675.837364	127406.295834	56.846797
2675.212382	127193.956410	56.851802
2674.743250	126978.736389	56.856807
2673.626264	126766.859218	56.861812
2672.994233	126556.418146	56.866817
2672.367349	126353.902607	56.871821
2671.881095	126141.384242	56.876826
2670.983408	125931.739350	56.881831
2670.339708	125730.831251	56.886836
2669.718632	125510.109817	56.891841
2668.820708	125310.908730	56.896845
2668.148310	125113.895750	56.901850
2667.527177	124894.538149	56.906855
2666.921326	124694.152382	56.911860
2666.288996	124493.658002	56.916865
2665.482662	124286.487642	56.921869
2664.806709	124083.577720	56.926874
2664.200548	123886.829856	56.931879
2663.317880	123690.355815	56.936884
2663.314990	123476.651564	56.941889
2662.079862	123276.731594	56.946893
2661.244884	123070.260853	56.951898
2660.906376	122873.478004	56.956903
2660.225375	122671.976358	56.961908
2659.805677	122459.285924	56.966913
2658.877208	122263.743869	56.971917
2658.512290	122056.698566	56.976922
2657.860976	121871.845181	56.981927
2656.811224	121656.416687	56.986932
2656.447977	121457.540399	56.991937
2655.649288	121250.214581	56.996941
2655.052772	121047.734152	57.001946
2654.675970	120847.404395	57.006951
2653.692153	120636.468603	57.011956
2653.327173	120434.578354	57.016961
2652.235530	120222.342466	57.021965
2651.685461	120021.805200	57.026970
2651.020267	119819.700607	57.031975
2650.141835	119619.485078	57.036980
2649.544484	119413.919363	57.041985
2649.269402	119219.159713	57.046989
2648.502145	119010.805467	57.051994
2647.891829	118803.526249	57.056999
2646.997869	118601.733949	57.062004
2646.623564	118397.670796	57.067009
2645.976108	118191.367246	57.072013
2645.261338	117985.863149	57.077018
2644.708194	117778.100611	57.082023
2643.794568	117584.146310	57.087028
2643.580671	117374.651078	57.092033
2642.854062	117161.969695	57.097037
2641.937484	116962.453559	57.102042
2641.488634	116749.433230	57.107047
2639.981592	116558.976670	57.112052
2639.753475	116340.243656	57.117057
2639.070265	116138.526085	57.122061
2638.323686	115932.262678	57.127066
2638.108435	115729.242779	57.132071
2637.128950	115542.766179	57.137076
2636.432790	115335.553848	57.142081
2635.733746	115129.575027	57.147085
2634.818382	114929.566780	57.152090
2634.625188	114721.422884	57.157095
2633.724408	114531.386830	57.162100
2633.343731	114323.859838	57.167105
2632.437647	114114.850094	57.172109
2631.962269	113915.694100	57.177114
2631.164711	113707.559103	57.182119
2630.453163	113515.552211	57.187124
2629.794498	113313.815118	57.192129
2629.446358	113114.207370	57.197133
2628.747722	112906.425091	57.202138
2627.876783	112701.413583	57.207143
2627.291220	112500.807490	57.212148
2626.634534	112291.075267	57.217153
2625.979425	112092.158959	57.222157
2625.248702	111891.549028	57.227162
2624.777799	111678.752573	57.232167
2623.925287	111492.374698	57.237172
2623.430468	111290.685085	57.242177
2622.560318	111085.800972	57.247181
2622.041603	110881.992482	57.252186
2621.711085	110675.211247	57.257191
2620.730170	110469.753249	57.262196
2620.103976	110262.273486	57.267201
2619.614857	110065.174779	57.272205
2619.021164	109853.079794	57.277210
2618.426820	109645.746131	57.282215
2617.452043	109445.486615	57.287220
2616.812704	109245.384988	57.292225
2616.115275	109038.415463	57.297229
2615.428029	108826.705876	57.302234
2614.730458	108630.647986	57.307239
2613.887614	108430.997732	57.312244
2613.423164	108213.534480	57.317249
2612.421275	108025.512299	57.322253
2611.790419	107825.173493	57.327258
2611.520739	107616.130421	57.332263
2610.707057	107417.575260	57.337268
2609.987406	107207.261817	57.342273
2608.961322	107015.101527	57.347277
2608.390993	106822.997445	57.352282
2608.014746	106622.742447	57.357287
2607.465820	106412.040856	57.362292
2606.713510	106212.914817	57.367297
2605.964519	106020.705851	57.372301
2605.208347	105824.933749	57.377306
2604.719856	105613.169988	57.382311
2603.604744	105415.224742	57.387316
2603.265727	105216.396781	57.392321
2602.591442	105019.736369	57.397325
2601.910487	104822.507619	57.402330
2601.322572	104626.318949	57.407335
2600.292310	104431.185388	57.412340
2599.970165	104228.175623	57.417345
2599.103219	104031.287432	57.422349
2598.505672	103835.265420	57.427354
2598.175478	103643.833982	57.432359
2597.388758	103430.969518	57.437364
2596.619002	103243.931385	57.442369
2596.342572	103037.022906	57.447373
2595.084750	102839.921080	57.452378
2594.659585	102641.610467	57.457383
2594.052118	102438.667607	57.462388
2593.687459	102240.420567	57.467393
2592.996044	102042.791584	57.472397
2591.971751	101846.270087	57.477402
2591.663471	101641.148845	57.482407
2590.813486	101453.217821	57.487412
2590.327665	101231.235071	57.492417
2589.381307	101039.180261	57.497421
2588.647744	100842.627470	57.502426
2588.413073	100637.198884	57.507431
2587.400496	100451.889828	57.512436
2586.833542	100237.262390	57.517441
2586.261032	100042.365482	57.522445
2585.562528	99843.614453	57.527450
2585.092002	99640.591744	57.532455
2583.762703	99453.970726	57.537460
2583.324001	99240.435901	57.542465
2582.609858	99052.845291	57.547469
2582.181944	98849.359739	57.552474
2581.802573	98642.690488	57.557479
2580.476095	98463.790032	57.562484
2580.138340	98262.553442	57.567489
2579.512171	98053.524673	57.572493
2578.436289	97861.852943	57.577498
2578.061206	97660.646576	57.582503
2577.081687	97476.903796	57.587508
2576.563232	97273.059670	57.592513
2575.627222	97088.120726	57.597517
2575.147314	96896.242138	57.602522
2574.553380	96699.353728	57.607527
2573.715265	96509.970639	57.612532
2573.089330	96314.466918	57.617537
2572.760500	96131.158281	57.622541
2572.283489	95943.079928	57.627546
2571.958220	95746.214282	57.632551
2570.641504	95545.784686	57.637556
2569.870713	95353.692530	57.642561
2569.097876	95166.593450	57.647565
2568.588111	94963.466303	57.652570
2568.160611	94765.731197	57.657575
2567.276781	94585.383228	57.662580
2566.511664	94371.539878	57.667585
2566.155722	94192.912448	57.672589
2565.513807	94006.614001	57.677594
2564.825534	93801.990970	57.682599
2563.939624	93613.527598	57.687604
2563.520928	93416.931773	57.692609
2562.509506	93227.698865	57.697613
2561.853520	93034.485935	57.702618
2561.540323	92840.744756	57.707623
2560.673257	92658.317040	57.712628
2560.111148	92462.957193	57.717633
2559.641656	92272.999711	57.722637
2558.533868	92080.335920	57.727642
2558.081009	91895.965522	57.732647
2557.318385	91699.173063	57.737652
2556.757730	91506.662166	57.742657
2556.424911	91306.875576	57.747661
2555.500528	91110.855874	57.752666
2554.904392	90915.591166	57.757671
2553.836396	90731.797193	57.762676
2553.417354	90534.535842	57.767681
2552.806234	90338.752355	57.772685
2551.962687	90157.222905	57.777690
2551.702842	89953.670761	57.782695
2550.760872	89763.632244	57.787700
2550.135023	89568.834391	57.792705
2549.658636	89383.112916	57.797709
2549.062188	89186.487804	57.802714
2548.353627	88987.016470	57.807719
2547.602084	88798.034008	57.812724
2547.069228	88604.307850	57.817729
2546.428613	88408.679471	57.822733
2545.640078	88206.679279	57.827738
2545.210710	88012.555258	57.832743
2544.527278	87817.756840	57.837748
2543.650277	87626.091011	57.842753
2542.738344	87428.327255	57.847757
2541.999617	87233.175163	57.852762
2541.939796	87042.507113	57.857767
2540.725421	86850.197947	57.862772
2540.069843	86665.364963	57.867777
2539.599086	86468.674858	57.872781
2538.889884	86277.805870	57.877786
2538.177753	86085.100636	57.882791
2537.553861	85896.243768	57.887796
2537.095979	85708.325815	57.892801
2536.218254	85515.962568	57.897805
2535.297905	85331.671158	57.902810
2535.272917	85134.713449	57.907815
2534.320638	84946.690382	57.912820
2533.788498	84750.101860	57.917825
2533.218599	84557.977373	57.922829
2532.084964	84363.421120	57.927834
2531.811891	84172.470123	57.932839
2530.760890	83970.164741	57.937844
2530.459401	83785.852016	57.942849
2530.060904	83585.247062	57.947853
2529.052814	83405.866972	57.952858
2528.519015	83203.670755	57.957863
2527.489509	83007.779372	57.962868
2526.711353	82822.289251	57.967873
2526.308847	82624.013903	57.972877
2525.640782	82447.560733	57.977882
2525.046419	82249.870747	57.982887
2524.398809	82058.136228	57.987892
2523.747084	81855.686429	57.992897
2523.067768	81669.303486	57.997901
2522.149361	81486.629777	58.002906
2521.792749	81280.386688	58.007911
2520.815078	81100.869341	58.012916
2519.906361	80908.565628	58.017921
2519.446750	80728.411644	58.022925
2518.958045	80533.947022	58.027930
2518.349200	80348.211141	58.032935
2517.489781	80167.897224	58.037940
2516.501038	79973.814963	58.042945
2516.241234	79792.344562	58.047949
2515.478886	79600.606449	58.052954
2515.240357	79413.907643	58.057959
2514.139051	79225.268652	58.062964
2513.615643	79035.703268	58.067969
2512.732598	78860.474248	58.072973
2511.939784	78669.725518	58.077978
2511.618660	78480.095150	58.082983
2511.100096	78305.186961	58.087988
2510.523989	78109.472553	58.092993
2509.662058	77933.056733	58.097997
2508.879076	77748.163924	58.103002
2508.534205	77551.207849	58.108007
2507.596619	77365.126341	58.113012
2507.034672	77171.218260	58.118017
2506.416735	76983.036487	58.123021
2505.912255	76795.617854	58.128026
2505.095895	76600.437517	58.133031
2504.273128	76428.159836	58.138036
2503.872347	76223.019767	58.143041
2503.270886	76047.573734	58.148045
2502.400868	75867.172493	58.153050
2501.880666	75665.934747	58.158055
2500.990171	75480.160780	58.163060
2500.399572	75282.004680	58.168065
2499.751203	75096.043788	58.173069
2498.963172	74908.864900	58.178074
2498.520806	74721.563256	58.183079
2497.446401	74545.147103	58.188084
2497.137184	74342.577549	58.193089
2496.332116	74166.172703	58.198093
2495.773542	73985.453766	58.203098
2495.075372	73797.770426	58.208103
2494.371427	73611.939728	58.213108
2493.487429	73418.923191	58.218113
2493.099404	73235.333003	58.223117
2492.283904	73046.528575	58.228122
2492.052510	72869.207915	58.233127
2491.227506	72686.654988	58.238132
2490.459610	72495.428152	58.243137
2489.698551	72307.033861	58.248141
2489.018170	72112.546906	58.253146
2488.632561	71927.207198	58.258151
2487.742504	71746.580017	58.263156
2487.109917	71556.284647	58.268161
2486.704537	71379.568606	58.273165
2486.134154	71187.942924	58.278170
2485.453117	70989.463485	58.283175
2484.168566	70813.994085	58.288180
2483.689204	70626.350226	58.293185
2483.320282	70435.219321	58.298189
2482.421275	70256.919227	58.303194
2482.250037	70062.568019	58.308199
2480.932953	69877.439468	58.313204
2480.154528	69687.210518	58.318209
2479.665372	69506.901277	58.323213
2478.902120	69333.243672	58.328218
2478.741368	69143.105756	58.333223
2477.949693	68967.954702	58.338228
2477.095406	68772.806069	58.343233
2476.715036	68583.367122	58.348237
2475.463135	68404.398699	58.353242
2475.186929	68215.326832	58.358247
2474.398641	68036.965995	58.363252
2474.008296	67848.846827	58.368257
2473.365891	67672.923659	58.373261
2472.469301	67479.156375	58.378266
2471.903747	67293.515095	58.383271
2471.191326	67115.106330	58.388276
2470.408120	66930.972373	58.393281
2469.947718	66752.989318	58.398285
2469.144459	66562.218375	58.403290
2468.484592	66370.115604	58.408295
2468.057359	66200.891180	58.413300
2467.329936	66011.985078	58.418305
2466.710698	65831.150947	58.423309
2466.011566	65646.468063	58.428314
2465.441563	65450.674391	58.433319
2464.693882	65271.775232	58.438324
2463.867153	65080.848477	58.443329
2463.376052	64894.819429	58.448333
2462.333242	64719.363365	58.453338
2461.960499	64535.402477	58.458343
2461.246007	64353.327633	58.463348
2460.950044	64167.271527	58.468353
2459.975624	63976.724281	58.473357
2459.297727	63799.474201	58.478362
2458.518721	63610.359233	58.483367
2458.105630	63430.442690	58.488372
2457.405124	63246.042733	58.493377
2456.873936	63054.272463	58.498381
2456.258943	62872.746835	58.503386
2455.441644	62680.180359	58.508391
2454.761123	62492.514054	58.513396
2454.405297	62312.466015	58.518401
2453.512009	62115.811087	58.523405
2452.393855	61942.311027	58.528410
2452.055499	61743.336881	58.533415
2451.137297	61574.417951	58.538420
2450.681521	61393.324439	58.543425
2450.193147	61205.143386	58.548429
2449.440587	61023.755398	58.553434
2448.609106	60838.946896	58.558439
2447.820789	60657.153397	58.563444
2447.547881	60473.887066	58.568449
2446.820132	60295.097969	58.573453
2445.632560	60111.404038	58.578458
2445.513269	59923.826204	58.583463
2444.697583	59746.509248	58.588468
2444.242969	59560.561459	58.593473
2443.635488	59378.435113	58.598477
2442.803088	59183.789018	58.603482
2442.120922	58995.600655	58.608487
2441.378701	58815.574470	58.613492
2440.556827	58630.735544	58.618497
2440.146616	58454.100905	58.623501
2439.137448	58280.705996	58.628506
2438.863202	58091.977788	58.633511
2437.874907	57908.938600	58.638516
2437.142090	57728.513116	58.643521
2436.709426	57561.446129	58.648525
2435.961784	57379.649552	58.653530
2435.606263	57189.832436	58.658535
2434.809679	57021.334097	58.663540
2434.115531	56835.688849	58.668545
2433.697029	56650.321424	58.673549
2432.610437	56476.980968	58.678554
2431.734626	56282.349980	58.683559
2431.516609	56108.859448	58.688564
2431.095323	55928.354644	58.693569
2430.066841	55737.912226	58.698573
2429.278185	55566.875060	58.703578
2428.711182	55378.765271	58.708583
2427.894312	55203.428723	58.713588
2427.110913	55024.449140	58.718593
2426.733486	54849.049470	58.723597
2425.933007	54674.626802	58.728602
2425.558971	54484.685411	58.733607
2424.700048	54309.728009	58.738612
2423.923472	54134.876314	58.743617
2423.670632	53947.041536	58.748621
2422.784463	53778.251685	58.753626
2422.106338	53587.269759	58.758631
2421.358069	53409.085201	58.763636
2420.763159	53226.932082	58.768641
2420.628318	53054.204075	58.773645
2419.596126	52878.313260	58.778650
2419.052419	52686.357522	58.783655
2418.339408	52508.742608	58.788660
2417.636872	52314.635809	58.793665
2417.156684	52145.037342	58.798669
2416.058547	51958.686086	58.803674
2415.680487	51778.664757	58.808679
2415.033660	51606.208909	58.813684
2414.436849	51421.343611	58.818689
2413.930854	51233.149895	58.823693
2412.948076	51064.043096	58.828698
2412.437526	50863.311836	58.833703
2411.844243	50686.926637	58.838708
2411.082430	50494.864237	58.843713
2410.394675	50317.959772	58.848717
2409.767962	50133.270639	58.853722
2409.030344	49948.487095	58.858727
2408.042192	49771.274978	58.863732
2407.148581	49597.007733	58.868737
2406.810221	49418.996888	58.873741
2406.174927	49242.322516	58.878746
2405.554485	49055.697839	58.883751
2404.766326	48881.034891	58.888756
2404.095413	48706.275974	58.893761
2403.520600	48529.580089	58.898765
2402.869395	48348.184409	58.903770
2402.572814	48164.611644	58.908775
2401.591036	47996.020869	58.913780
2400.847987	47810.766826	58.918785
2400.274381	47638.543211	58.923789
2399.423876	47461.164589	58.928794
2398.981768	47283.558495	58.933799
2398.305567	47103.065239	58.938804
2397.572893	46915.927250	58.943809
2396.733373	46747.654781	58.948813
2396.138725	46569.080463	58.953818
2395.663732	46391.137432	58.958823
2394.944528	46224.391345	58.963828
2394.464719	46039.952348	58.968833
2393.675519	45858.205516	58.973837
2392.959738	45681.902023	58.978842
2392.363110	45500.087239	58.983847
2391.915535	45334.574888	58.988852
2390.764308	45139.956264	58.993857
2390.312432	44966.543844	58.998861
2389.462562	44801.492516	59.003866
2389.142182	44610.135498	59.008871
2388.269433	44445.261953	59.013876
2387.667007	44271.016842	59.018881
2387.079685	44091.457628	59.023885
2386.254022	43910.464219	59.028890
2385.498268	43724.546769	59.033895
2384.956821	43559.549993	59.038900
2384.393396	43379.557873	59.043905
2383.854024	43203.899732	59.048909
2382.727767	43041.195452	59.053914
2382.481074	42854.896643	59.058919
2381.667844	42672.680751	59.063924
2381.089403	42504.176828	59.068929
2380.555118	42317.072365	59.073933
2379.476005	42148.847360	59.078938
2378.919370	41970.529047	59.083943
2378.156591	41796.587164	59.088948
2377.613983	41617.726343	59.093953
2377.299841	41447.087869	59.098957
2376.470092	41277.415109	59.103962
2376.129598	41090.261580	59.108967
2375.289021	40915.683176	59.113972
2374.494860	40744.795742	59.118977
2373.939868	40556.502545	59.123981
2373.086839	40379.490404	59.128986
2372.690886	40209.901683	59.133991
2372.078896	40028.330040	59.138996
2370.955850	39847.764660	59.144001
2370.695310	39668.073081	59.149005
2369.817918	39487.244890	59.154010
2369.321993	39302.944862	59.159015
2368.771646	39133.370732	59.164020
2368.002445	38952.333431	59.169025
2367.515572	38768.757047	59.174029
2366.910404	38595.709500	59.179034
2365.927468	38401.745573	59.184039
2365.235518	38225.986978	59.189044
2364.621632	38054.879686	59.194049
2364.100430	37875.678304	59.199053
2363.201235	37704.758893	59.204058
2362.372226	37519.071914	59.209063
2362.011982	37337.462135	59.214068
2361.155255	37157.411029	59.219073
2360.581760	36979.074696	59.224077
2359.766019	36812.197725	59.229082
2359.237699	36633.156040	59.234087
2358.531139	36459.531474	59.239092
2357.964884	36288.432895	59.244097
2357.523202	36102.306470	59.249101
2356.457586	35925.875464	59.254106
2356.262827	35743.783966	59.259111
2355.275385	35575.601362	59.264116
2354.443574	35400.521814	59.269121
2353.955292	35213.533806	59.274125
2353.329048	35040.556013	59.279130
2352.791212	34864.694160	59.284135
2351.950899	34691.237084	59.289140
2351.259925	34512.253251	59.294145
2350.746791	34333.472300	59.299149
2349.993956	34159.810882	59.304154
2349.406947	33980.093985	59.309159
2348.716390	33803.640067	59.314164
2347.836725	33623.383922	59.319169
2347.545469	33455.847111	59.324173
2346.694771	33273.101036	59.329178
2346.067463	33091.138589	59.334183
2345.515727	32924.481283	59.339188
2344.445354	32736.616109	59.344193
2344.011681	32562.272799	59.349197
2343.077131	32398.764666	59.354202
2342.434097	32226.866454	59.359207
2341.769112	32053.118276	59.364212
2340.987256	31871.476579	59.369217
2340.737630	31702.346905	59.374221
2339.915081	31539.107622	59.379226
2339.082429	31362.340316	59.384231
2338.335631	31198.463470	59.389236
2337.954180	31026.550475	59.394241
2337.371448	30847.353522	59.399245
2336.782319	30680.988624	59.404250
2336.165858	30497.727243	59.409255
2335.336310	30328.841086	59.414260
2334.373217	30161.034919	59.419265
2334.188017	29982.098784	59.424269
2333.234902	29813.610418	59.429274
2332.726908	29634.073547	59.434279
2331.790764	29463.715329	59.439284
2331.167256	29298.073001	59.444289
2330.554503	29119.275706	59.449293
2329.845834	28958.532469	59.454298
2329.312424	28775.522059	59.459303
2328.577096	28614.429367	59.464308
2327.962311	28434.344345	59.469313
2327.556579	28254.766903	59.474317
2326.629190	28097.542611	59.479322
2325.996086	27920.151979	59.484327
2325.515204	27752.881773	59.489332
2324.613186	27576.676605	59.494337
2324.192195	27395.788741	59.499341
2323.316111	27233.596152	59.504346
2322.807332	27055.950368	59.509351
2321.846911	26888.017885	59.514356
2321.112647	26714.729102	59.519361
2320.658434	26544.076987	59.524365
2319.883394	26377.411834	59.529370
2319.331155	26205.455035	59.534375
2318.830921	26034.953024	59.539380
2318.298159	25862.958870	59.544385
2317.670157	25692.332253	59.549389
2316.670718	25524.653129	59.554394
2316.067423	25350.460193	59.559399
2315.340506	25176.756310	59.564404
2314.302488	25011.765279	59.569409
2313.895426	24838.676956	59.574413
2313.011156	24689.635844	59.579418
2312.931350	24510.950189	59.584423
2312.126776	24353.384300	59.589428
2311.592039	24166.880199	59.594433
2310.977884	23997.274735	59.599437
2310.413521	23828.711937	59.604442
2309.532684	23656.956917	59.609447
2308.986496	23489.704173	59.614452
2308.483570	23312.074297	59.619457
2307.804858	23139.381465	59.624461
2306.425555	22961.886583	59.629466
2306.243503	22790.194321	59.634471
2305.277421	22631.050608	59.639476
2304.362458	22459.031990	59.644481
2304.264168	22287.061013	59.649485
2303.293819	22133.153647	59.654490
2302.855531	21952.910992	59.659495
2302.189162	21787.897488	59.664500
2301.456324	21626.438494	59.669505
2300.953001	21452.599106	59.674509
2299.620692	21284.259271	59.679514
2299.211077	21108.861165	59.684519
2298.754040	20943.262644	59.689524
2298.004206	20781.889973	59.694529
2297.687688	20602.722728	59.699533
2296.786740	20440.278429	59.704538
2296.219131	20272.987171	59.709543
2295.390260	20098.508446	59.714548
2294.617955	19937.996736	59.719553
2293.927877	19765.731320	59.724557
2293.222105	19608.477130	59.729562
2292.730781	19444.097499	59.734567
2292.149349	19280.231662	59.739572
2291.420788	19108.006402	59.744577
2291.128099	18934.137292	59.749581
2289.816266	18774.428848	59.754586
2289.156337	18606.046148	59.759591
2288.447399	18443.606251	59.764596
2287.992813	18291.289186	59.769601
2287.411157	18122.161137	59.774605
2286.674392	17964.292854	59.779610
2286.330457	17796.013619	59.784615
2285.557071	17625.325523	59.789620
2284.732049	17456.417353	59.794625
2284.005449	17288.190081	59.799629
2283.207402	17129.820932	59.804634
2282.587821	16969.308735	59.809639
2282.185644	16799.670827	59.814644
2281.445990	16638.712194	59.819649
2280.837683	16474.294345	59.824653
2279.815734	16313.004574	59.829658
2279.277381	16147.902215	59.834663
2278.736334	15992.525722	59.839668
2277.681708	15830.009267	59.844673
2277.420808	15671.340698	59.849677
2276.833401	15521.041184	59.854682
2276.238070	15347.029238	59.859687
2275.588550	15178.667779	59.864692
2274.746592	15021.117622	59.869697
2274.350966	14859.150221	59.874701
2273.649194	14690.382676	59.879706
2272.857299	14521.550669	59.884711
2272.160732	14357.447050	59.889716
2271.474128	14194.546710	59.894721
2270.918834	14035.123207	59.899725
2269.897488	13884.333319	59.904730
2269.299124	13718.108468	59.909735
2268.588817	13557.309421	59.914740
2267.907235	13394.353831	59.919745
2267.706760	13236.922929	59.924750
2266.947045	13075.172154	59.929754
2266.073290	12913.880946	59.934759
2265.689937	12755.930458	59.939764
2264.995674	12598.430456	59.944769
2264.165942	12433.753090	59.949774
2263.451943	12273.584027	59.954778
2262.644274	12103.696167	59.959783
2261.884112	11951.445691	59.964788
2261.290232	11797.294807	59.969793
2260.828364	11635.510357	59.974798
2259.822438	11492.823154	59.979802
2259.287176	11325.070227	59.984807
2258.745171	11166.912026	59.989812
2257.756945	11019.366246	59.994817
2257.260922	10854.212522	59.999822
2256.571115	10698.812054	60.004826
2255.997679	10543.180884	60.009831
2255.169916	10385.645457	60.014836
2254.558229	10226.572689	60.019841
2253.817162	10076.804325	60.024846
2252.996989	9925.965868	60.029850
2252.654946	9776.305051	60.034855
2251.861259	9616.052087	60.039860
2251.022650	9466.851236	60.044865
2250.636210	9319.929370	60.049870
2249.895561	9174.579189	60.054874
2248.840756	9017.116925	60.059879
2248.244042	8859.220717	60.064884
2247.726384	8714.383206	60.069889
2247.177323	8562.618325	60.074894
2246.257961	8434.315914	60.079898
2245.789112	8276.316388	60.084903
2245.351802	8124.419863	60.089908
2244.459389	7973.479083	60.094913
2243.736447	7825.170014	60.099918
2242.931228	7681.857430	60.104922
2242.491359	7521.952085	60.109927
2241.783917	7385.263859	60.114932
2240.987646	7249.717503	60.119937
2240.444368	7087.360040	60.124942
2239.437344	6949.734063	60.129946
2238.902081	6804.066203	60.134951
2238.356044	6657.184267	60.139956
2237.414479	6516.889901	60.144961
2236.978520	6376.155756	60.149966
2236.005689	6251.924533	60.154970
2235.218068	6107.715516	60.159975
2234.259172	5976.175902	60.164980
2233.338874	5843.803864	60.169985
2232.923689	5702.317107	60.174990
2232.013976	5578.357578	60.179994
2231.028810	5453.453459	60.184999
2230.179582	5341.241692	60.190004
2229.055073	5224.501883	60.195009
2227.989260	5123.466070	60.200014
2226.980066	5029.377336	60.205018
2226.164071	4939.525770	60.210023
2225.067721	4859.734906	60.215028
2223.660847	4784.981041	60.220033
2223.011881	4704.575802	60.225038
2222.437083	4642.104847	60.230042
2221.460170	4569.333038	60.235047
2220.943271	4498.707344	60.240052
2219.810264	4445.078442	60.245057
2219.414363	4369.044722	60.250062
2218.079514	4320.563239	60.255066
2217.860382	4268.001500	60.260071
2217.130542	4211.198745	60.265076
2216.142133	4163.422366	60.270081
2215.788247	4103.929201	60.275086
2215.127854	4064.075864	60.280090
2214.462854	3998.633488	60.285095
2213.877066	3940.968152	60.290100
2213.244040	3901.634618	60.295105
2212.887199	3834.729139	60.300110
2212.005145	3784.338332	60.305114
2211.275742	3731.308939	60.310119
2210.625382	3671.902408	60.315124
2209.680917	3635.288734	60.320129
2209.629147	3585.998045	60.325134
2208.978995	3526.914642	60.330138
2208.416549	3475.263554	60.335143
2207.493070	3420.657148	60.340148
2207.010644	3373.678507	60.345153
2206.633588	3306.109044	60.350158
2205.651406	3271.563078	60.355162
2205.281768	3200.278262	60.360167
2204.915465	3147.117661	60.365172
2203.939341	3104.037729	60.370177
2203.381711	3037.605436	60.375182
2202.601914	2980.197837	60.380186
2202.117873	2918.781329	60.385191
2201.261496	2864.043320	60.390196
2200.329566	2812.920849	60.395201
2200.088553	2754.725970	60.400206
2199.232958	2712.602049	60.405210
2198.894043	2647.410487	60.410215
2198.320085	2593.222534	60.415220
2197.242966	2538.508143	60.420225
2196.932682	2486.941978	60.425230
2196.256151	2430.341118	60.430234
2195.558126	2377.500911	60.435239
2195.203519	2320.441683	60.440244
2194.151800	2265.485331	60.445249
2193.814796	2203.682570	60.450254
2192.992901	2155.654464	60.455258
2192.213714	2102.425933	60.460263
2191.778497	2038.492845	60.465268
2191.007018	1991.133909	60.470273
2190.612205	1932.379968	60.475278
2189.732577	1880.413386	60.480282
2189.021550	1818.514658	60.485287
2188.365165	1767.151038	60.490292
2187.385099	1712.061592	60.495297
2187.074977	1659.034690	60.500302
2186.453515	1624.291084	60.505306
2185.960417	1561.657027	60.510311
2185.531011	1514.631774	60.515316
2184.484008	1455.148114	60.520321
2183.739720	1399.848167	60.525326
2183.176526	1345.108762	60.530330
2182.794580	1294.452410	60.535335
2181.912697	1239.717436	60.540340
2180.987864	1194.328447	60.545345
2180.793436	1123.851561	60.550350
2179.644001	1077.461613	60.555354
2179.226162	1026.091934	60.560359
2178.454458	971.042416	60.565364
2177.698957	922.134914	60.570369
2177.418967	864.196609	60.575374
2176.486959	818.451932	60.580378
2175.778260	771.294388	60.585383
2175.181282	727.088910	60.590388
2174.392975	675.310852	60.595393
2174.141128	616.075081	60.600398
2173.198416	582.199487	60.605402
2172.103086	520.935773	60.610407
2171.628220	476.475126	60.615412
2170.961202	440.099078	60.620417
2170.248048	387.838586	60.625422
2169.484505	352.438491	60.630426
2168.886698	296.379868	60.635431
2168.390381	260.642696	60.640436
2167.448446	209.366937	60.645441
2166.913834	177.805692	60.650446
2166.284578	131.842464	60.655450
2165.280768	93.558917	60.660455
2164.755652	49.500226	60.665460
2163.949020	23.700696	60.670465
2163.415742	-24.263498	60.675470
2162.259513	-41.978950	60.680474
2161.727321	-79.680835	60.685479
2161.216714	-121.279625	60.690484
2160.173492	-127.972414	60.695489
2159.600013	-166.350356	60.700494
2156.593655	-140.972802	60.705498
2148.488269	55.199016	60.710503
2150.109532	59.527718	60.715508
2151.677971	74.418133	60.720513
2154.091748	68.351630	60.725518
2155.085044	64.327218	60.730522
2154.759701	53.264107	60.735527
2154.710772	32.278799	60.740532
2153.396127	28.021318	60.745537
2152.515017	27.501935	60.750542
2150.861146	32.577361	60.755546
2149.482840	37.169083	60.760551
2149.134863	42.888897	60.765556
2148.285163	48.038593	60.770561
2147.960647	44.511865	60.775566
2147.756395	45.356436	60.780570
2146.646325	44.296199	60.785575
2146.634064	45.397322	60.790580
2145.791527	50.987444	60.795585
2145.324559	41.031795	60.800590
2144.351237	50.067921	60.805594
2143.288324	50.851606	60.810599
2143.459821	49.023462	60.815604
2142.840117	51.357987	60.820609
2142.533983	48.799777	60.825614
2141.368621	53.936481	60.830618
2140.379708	48.442987	60.835623
2139.563152	46.025692	60.840628
2138.574849	49.644034	60.845633
2138.574875	45.277311	60.850638
2137.960913	50.839053	60.855642
2137.132112	53.848597	60.860647
2136.348309	54.423991	60.865652
2135.947081	56.351679	60.870657
2135.786748	51.407982	60.875662
2134.613339	54.418587	60.880666
2133.930432	59.912422	60.885671
2133.191804	52.169833	60.890676
2132.507644	57.067758	60.895681
2132.568820	56.465103	60.900686
2131.815226	52.000329	60.905690
2131.372191	60.944438	60.910695
2130.298665	51.655905	60.915700
2128.893329	56.799152	60.920705
2128.899928	51.239169	60.925710
2128.290675	60.370508	60.930714
2127.239604	60.289699	60.935719
2126.736634	54.889419	60.940724
2125.681564	64.015803	60.945729
2125.745068	56.751507	60.950734
2125.345315	57.740645	60.955738
2124.662974	65.571516	60.960743
2124.015195	52.969953	60.965748
2123.206861	57.013922	60.970753
2122.372614	54.626247	60.975758
2121.613388	56.270109	60.980762
2120.756876	64.469250	60.985767
2120.364465	59.362097	60.990772
2119.360573	66.763005	60.995777
2118.575185	57.362519	61.000782
2117.755662	59.624674	61.005786
2117.494764	52.459166	61.010791
2117.470937	66.706464	61.015796
2116.580347	70.235194	61.020801
2116.173223	65.527780	61.025806
2115.398894	60.681509	61.030810
2114.698897	64.660983	61.035815
2113.611588	63.920433	61.040820
2113.015272	69.820019	61.045825
2112.433884	59.365265	61.050830
2111.716466	60.966225	61.055834
2110.940569	68.547008	61.060839
2110.442431	64.675658	61.065844
2109.586029	72.179328	61.070849
2109.044839	66.565909	61.075854
2108.534914	71.172837	61.080858
2107.604590	68.633247	61.085863
2107.483912	66.250622	61.090868
2106.962398	72.775452	61.095873
2105.551464	69.211375	61.100878
2105.318273	60.786172	61.105882
2104.976303	68.201904	61.110887
2103.879321	64.699979	61.115892
2103.132635	71.274731	61.120897
2103.017894	64.909225	61.125902
2102.019978	65.312017	61.130906
2101.152449	66.588282	61.135911
2101.120971	66.142259	61.140916
2099.676415	62.279161	61.145921
2099.828366	59.318672	61.150926
2098.515618	63.572006	61.155930
2097.746833	66.116285	61.160935
2097.586504	63.109151	61.165940
2097.133484	66.054347	61.170945
2096.551758	64.345723	61.175950
2095.279615	63.453156	61.180954
2094.351462	67.766893	61.185959
2094.169610	66.079974	61.190964
2093.283836	70.035315	61.195969
2093.076486	64.422545	61.200974
2091.820037	63.581107	61.205978
2091.603286	71.588848	61.210983
2091.288754	57.508799	61.215988
2089.894527	71.418453	61.220993
2089.637121	65.924016	61.225998
2088.653256	60.194765	61.231002
2087.984127	67.667144	61.236007
2087.631218	64.804115	61.241012
2087.103819	78.475295	61.246017
2086.363150	59.162549	61.251022
2085.534661	62.137365	61.256026
2084.766136	71.275067	61.261031
2084.476580	67.566171	61.266036
2083.252082	68.493798	61.271041
2082.819378	69.514980	61.276046
2082.269046	67.263619	61.281050
2081.477963	69.298914	61.286055
2081.179755	65.566161	61.291060
2080.281440	70.491777	61.296065
2079.941130	75.480238	61.301070
2079.058474	69.208207	61.306074
2078.534910	75.862681	61.311079
2078.308648	66.392402	61.316084
2077.854698	75.218403	61.321089
2077.066255	68.283273	61.326094
2075.768138	67.574615	61.331098
2074.591000	75.707955	61.336103
2074.218765	64.000993	61.341108
2073.230163	77.497773	61.346113
2072.662507	65.252523	61.351118
2072.714786	71.208467	61.356122
2071.672769	69.902487	61.361127
2071.432752	70.025740	61.366132
2070.469004	67.797408	61.371137
2069.814609	69.965562	61.376142
2069.440166	72.887255	61.381146
2068.514081	73.062611	61.386151
2068.109558	61.488514	61.391156
2067.285716	68.843518	61.396161
2066.663080	66.094262	61.401166
2066.536164	65.704387	61.406170
2064.793249	70.738810	61.411175
2063.924088	63.557867	61.416180
2063.516946	67.235403	61.421185
2063.788391	63.391750	61.426190
2062.595960	54.166276	61.431194
2061.492528	66.550559	61.436199
2061.130412	58.962714	61.441204
2060.390531	74.952691	61.446209
2059.727069	69.025941	61.451214
2059.209648	61.469049	61.456218
2058.525700	62.186320	61.461223
2058.424989	65.280621	61.466228
2057.872105	70.788535	61.471233
2057.247862	70.534358	61.476238
2056.465080	58.946176	61.481242
2054.883801	62.669692	61.486247
2054.299275	61.076645	61.491252
2053.609008	68.273254	61.496257
2053.535466	63.370984	61.501262
2052.685004	60.497034	61.506266
2051.849585	62.998282	61.511271
2051.324603	60.682979	61.516276
2050.627506	72.617996	61.521281
2050.009598	64.063038	61.526286
2049.889425	62.864668	61.531290
2049.061751	69.922232	61.536295
2048.974255	60.511944	61.541300
2047.250286	67.814255	61.546305
2046.521120	63.295165	61.551310
2045.732245	63.527604	61.556314
2045.012295	69.457861	61.561319
2044.531790	61.109766	61.566324
2044.112253	61.750383	61.571329
2044.012391	67.951249	61.576334
2043.301446	64.004875	61.581338
2042.486131	66.783641	61.586343
2042.271883	62.348419	61.591348
2040.780532	62.692345	61.596353
2039.838745	61.906653	61.601358
2039.303806	57.224274	61.606362
2038.469544	61.841680	61.611367
2038.170102	55.732587	61.616372
2037.607917	66.688949	61.621377
2037.048627	60.124336	61.626382
2036.545907	61.074633	61.631386
2035.968218	62.997223	61.636391
2035.265964	60.957648	61.641396
2033.969698	66.763322	61.646401
2033.133326	57.104448	61.651406
2032.500208	63.576030	61.656410
2032.450734	66.643276	61.661415
2031.961284	65.654907	61.666420
2031.096250	63.153872	61.671425
2030.723850	66.256599	61.676430
2029.867163	71.765423	61.681434
2029.146417	71.512376	61.686439
2028.062171	53.328135	61.691444
2027.289226	67.113975	61.696449
2026.532089	65.086266	61.701454
2026.495704	60.837290	61.706458
2025.764275	70.538412	61.711463
2025.337849	57.299336	61.716468
2024.402227	68.594099	61.721473
2023.883725	60.364008	61.726478
2023.541540	65.261301	61.731482
2022.384480	73.009836	61.736487
2021.446868	57.319223	61.741492
2020.733516	65.317464	61.746497
2019.988964	61.163536	61.751502
2019.575584	65.094387	61.756506
2019.443675	62.946948	61.761511
2018.981798	57.783031	61.766516
2018.433724	61.858265	61.771521
2017.505932	66.359631	61.776526
2016.617374	62.096091	61.781530
2015.426937	71.078411	61.786535
2014.973333	59.654051	61.791540
2014.570833	62.133909	61.796545
2013.788831	60.971195	61.801550
2013.601401	61.007257	61.806554
2012.844579	60.487118	61.811559
2011.913450	57.586561	61.816564
2010.626967	65.771966	61.821569
2010.158719	61.545802	61.826574
2009.629016	62.232295	61.831578
2009.079777	68.126002	61.836583
2008.655750	63.211553	61.841588
2008.092098	67.803366	61.846593
2007.539218	62.958255	61.851598
2007.246565	64.800917	61.856602
2005.905310	62.206737	61.861607
2004.889225	62.364860	61.866612
2004.210211	72.253216	61.871617
2003.497425	63.257579	61.876622
2003.202853	66.142945	61.881626
2002.299089	78.796773	61.886631
2002.548891	65.038768	61.891636
2001.692732	71.873776	61.896641
2001.190114	67.222545	61.901646
2000.294954	66.858412	61.906650
1999.253921	70.472558	61.911655
1998.814271	62.376619	61.916660
1998.178415	74.470664	61.921665
1997.838295	67.571642	61.926670
1996.541532	63.998971	61.931674
1995.312454	76.106747	61.936679
1995.008778	68.416592	61.941684
1994.349395	66.769205	61.946689
1993.759441	73.766974	61.951694
1993.537391	67.502092	61.956698
1992.810369	72.649713	61.961703
1992.722271	69.834556	61.966708
1992.154018	74.610037	61.971713
1991.036642	68.264906	61.976718
1989.944770	70.199731	61.981722
1989.040545	77.419278	61.986727
1988.346996	63.158129	61.991732
1987.783081	72.018937	61.996737
1987.602251	68.985103	62.001742
1987.172431	55.431178	62.006746
1986.623268	73.844707	62.011751
1985.498405	68.276654	62.016756
1984.270401	62.009015	62.021761
1983.621263	59.923176	62.026766
1983.607421	59.687251	62.031770
1982.930264	61.906346	62.036775
1983.212352	60.475392	62.041780
1981.747393	64.898023	62.046785
1980.608524	63.720998	62.051790
1980.139147	65.728913	62.056794
1978.991894	72.895569	62.061799
1978.884546	65.488080	62.066804
1978.336082	67.254652	62.071809
1977.937665	64.950815	62.076814
1977.705785	66.736524	62.081818
1976.110153	74.732891	62.086823
1975.546129	61.315388	62.091828
1974.791524	63.988340	62.096833
1974.483283	67.033579	62.101838
1973.949179	65.202304	62.106842
1973.085020	63.147443	62.111847
1972.141705	60.960063	62.116852
1971.527782	65.635557	62.121857
1970.842877	61.543142	62.126862
1970.359876	69.232010	62.131866
1969.909310	71.555496	62.136871
1969.389553	64.897890	62.141876
1967.859159	62.362139	62.146881
1967.152499	66.243352	62.151886
1966.770863	63.574143	62.156890
1966.013440	69.959811	62.161895
1965.996091	61.908815	62.166900
1965.038495	68.920786	62.171905
1964.659279	68.222448	62.176910
1964.556373	64.105463	62.181914
1962.994507	68.685417	62.186919
1962.456286	63.150418	62.191924
1961.628922	63.605040	62.196929
1960.902120	63.657334	62.201934
1960.581958	55.417859	62.206938
1959.960620	67.649951	62.211943
1959.174054	67.593457	62.216948
1958.162951	58.818663	62.221953
1957.296193	61.468419	62.226958
1957.278249	54.945639	62.231962
1956.605725	67.214242	62.236967
1956.450656	58.973791	62.241972
1955.133261	64.708733	62.246977
1954.235174	65.453713	62.251982
1953.442256	58.185020	62.256986
1952.750919	64.593315	62.261991
1952.874833	61.364451	62.266996
1952.327922	67.803439	62.272001
1951.538091	60.874888	62.277006
1950.555586	57.624530	62.282010
1949.512178	64.747900	62.287015
1949.265566	60.160127	62.292020
1948.282810	63.566337	62.297025
1948.106112	65.601916	62.302030
1947.612573	63.732668	62.307034
1946.251974	68.143482	62.312039
1945.698526	57.638617	62.317044
1945.059093	59.865925	62.322049
1944.501753	62.766199	62.327054
1944.544249	70.340112	62.332058
1943.743872	71.326637	62.337063
1942.834728	57.669034	62.342068
1942.020230	65.684924	62.347073
1941.564692	61.917241	62.352078
1941.074171	64.264420	62.357082
1939.536989	71.838351	62.362087
1938.674319	59.707796	62.367092
1938.152751	59.716478	62.372097
1938.032537	54.343798	62.377102
1937.351282	52.461773	62.382106
1936.705706	63.428225	62.387111
1936.402896	60.866362	62.392116
1935.790802	59.246179	62.397121
1934.734387	56.851256	62.402126
1933.807346	54.139321	62.407130
1932.939528	66.741713	62.412135
1932.584603	65.627925	62.417140
1932.337512	62.435878	62.422145
1932.099730	57.643274	62.427150
1930.875570	52.486844	62.432154
1929.923639	59.390685	62.437159
1929.476308	53.875964	62.442164
1928.902224	60.355537	62.447169
1928.091943	65.849134	62.452174
1927.627062	57.549058	62.457178
1926.530127	76.625152	62.462183
1926.065170	56.568531	62.467188
1925.494478	67.307051	62.472193
1924.926153	65.708308	62.477198
1924.584027	52.108945	62.482202
1923.418754	62.855115	62.487207
1922.614575	60.401232	62.492212
1921.868112	59.903130	62.497217
1921.478836	60.863824	62.502222
1921.116513	59.746482	62.507226
1920.379181	59.805191	62.512231
1919.305078	53.122063	62.517236
1918.701024	61.934049	62.522241
1917.815924	63.973276	62.527246
1917.685991	63.348915	62.532250
1916.976192	58.601282	62.537255
1916.717132	57.328772	62.542260
1915.424185	58.445542	62.547265
1914.697891	54.951093	62.552270
1914.108356	51.796067	62.557274
1913.217757	54.082178	62.562279
1913.176450	54.836240	62.567284
1912.709049	56.053773	62.572289
1911.623649	64.071672	62.577294
1910.659617	56.369677	62.582298
1910.050195	55.865593	62.587303
1909.628713	44.410157	62.592308
1908.935107	50.817237	62.597313
1908.457299	52.194911	62.602318
1908.478986	46.896695	62.607322
1907.071335	56.265987	62.612327
1906.273912	44.335631	62.617332
1906.071381	58.709822	62.622337
1904.679217	53.398722	62.627342
1903.830957	48.505128	62.632346
1902.826747	59.876246	62.637351
1903.094800	52.598416	62.642356
1902.544928	50.677407	62.647361
1901.710047	51.784542	62.652366
1901.768377	49.099118	62.657370
1900.397866	63.548348	62.662375
1899.791160	50.244107	62.667380
1899.098189	54.510312	62.672385
1898.252281	57.353900	62.677390
1898.034788	51.909146	62.682394
1897.060610	54.715537	62.687399
1896.278311	56.208577	62.692404
1895.587445	57.310198	62.697409
1894.844631	56.494548	62.702414
1895.034026	53.988594	62.707418
1894.151337	58.216322	62.712423
1893.404074	61.652974	62.717428
1892.449547	64.108520	62.722433
1891.658935	60.108608	62.727438
1891.039539	59.836354	62.732442
1890.485008	61.919305	62.737447
1889.905030	50.683003	62.742452
1888.579568	62.672849	62.747457
1887.857722	58.892264	62.752462
1887.943536	56.432717	62.757466
1887.198364	58.623208	62.762471
1887.239542	51.290720	62.767476
1886.427087	59.803837	62.772481
1885.452416	55.975080	62.777486
1884.814134	48.733120	62.782490
1883.816264	57.570573	62.787495
1883.505106	51.574548	62.792500
1882.342746	59.026702	62.797505
1881.235185	64.715745	62.802510
1880.662151	55.514250	62.807514
1880.200007	57.673212	62.812519
1880.014708	55.991591	62.817524
1879.753499	56.826299	62.822529
1879.255144	60.731231	62.827534
1878.055512	57.211014	62.832538
1877.141131	55.865138	62.837543
1876.789532	65.541461	62.842548
1876.474679	57.042532	62.847553
1875.158244	58.040044	62.852558
1874.406733	53.060134	62.857562
1873.314323	55.256871	62.862567
1873.064998	53.102854	62.867572
1873.253993	50.535461	62.872577
1872.150260	51.776756	62.877582
1871.387570	56.259835	62.882586
1870.124719	67.380286	62.887591
1869.884684	53.033789	62.892596
1869.335525	43.974386	62.897601
1869.123995	55.184174	62.902606
1868.458826	54.417707	62.907610
1867.413022	62.933185	62.912615
1866.514256	63.027001	62.917620
1865.814215	61.996404	62.922625
1865.806719	57.787796	62.927630
1865.408191	59.244357	62.932634
1863.883545	62.779210	62.937639
1863.272940	50.617350	62.942644
1863.065661	57.898158	62.947649
1862.196673	52.283238	62.952654
1861.337868	49.995750	62.957658
1860.188037	59.355669	62.962663
1859.787894	60.783313	62.967668
1859.540172	53.110330	62.972673
1858.789794	49.662302	62.977678
1858.504514	50.781540	62.982682
1857.655444	65.646328	62.987687
1857.016165	47.603658	62.992692
1856.047002	64.472955	62.997697
1855.726008	65.973191	63.002702
1855.011022	54.545439	63.007706
1853.883707	62.359482	63.012711
1853.073686	56.217157	63.017716
1852.787105	55.575092	63.022721
1851.832216	56.483672	63.027726
1851.787562	52.338527	63.032730
1851.184047	58.879555	63.037735
1850.650131	53.077393	63.042740
1849.946590	49.967295	63.047745
1849.004783	56.076319	63.052750
1848.607341	51.583478	63.057754
1847.291423	60.303491	63.062759
1846.490209	50.869360	63.067764
1845.542106	55.930681	63.072769
1845.347151	57.073427	63.077774
1845.210664	50.858070	63.082778
1844.634378	56.174178	63.087783
1844.037511	50.814111	63.092788
1843.019085	51.229719	63.097793
1842.256579	55.039397	63.102798
1842.193198	50.529786	63.107802
1840.875342	64.147483	63.112807
1840.131729	54.968355	63.117812
1839.107361	54.430823	63.122817
1838.695148	57.364843	63.127822
1838.499923	49.558159	63.132826
1837.972297	53.040375	63.137831
1837.553856	53.543651	63.142836
1836.418778	50.830092	63.147841
1835.551588	52.730877	63.152846
1835.479064	52.083213	63.157850
1834.417259	61.458340	63.162855
1833.336296	50.515289	63.167860
1832.748218	54.401355	63.172865
1832.184057	53.916913	63.177870
1831.808639	51.737190	63.182874
1831.298038	56.951404	63.187879
1830.754820	47.859528	63.192884
1830.037625	48.090111	63.197889
1828.988061	57.097429	63.202894
1828.612736	47.917392	63.207898
1827.989744	57.249651	63.212903
1826.851303	49.748860	63.217908
1826.276668	58.295980	63.222913
1825.410512	63.095132	63.227918
1825.638371	47.780985	63.232922
1825.000179	53.923810	63.237927
1823.828789	63.270609	63.242932
1822.772131	49.981860	63.247937
1822.174753	53.028864	63.252942
1821.871193	56.339883	63.257946
1821.451359	55.900337	63.262951
1820.859788	43.911311	63.267956
1819.815050	50.703757	63.272961
1818.802521	57.434319	63.277966
1818.517947	48.231989	63.282970
1818.026405	55.874911	63.287975
1817.647105	45.265171	63.292980
1816.704584	48.400097	63.297985
1815.771110	57.202900	63.302990
1815.355910	46.644593	63.307994
1814.615009	56.670531	63.312999
1813.707278	50.852041	63.318004
1813.225882	53.142595	63.323009
1812.396179	55.302371	63.328014
1812.130543	56.781204	63.333018
1811.522827	59.317328	63.338023
1810.784187	60.324051	63.343028
1809.361185	54.398143	63.348033
1808.967597	57.974202	63.353038
1808.537299	53.456622	63.358042
1808.104165	61.358363	63.363047
1807.813669	61.786131	63.368052
1806.669344	59.692237	63.373057
1805.634296	64.451979	63.378062
1805.307241	49.691164	63.383066
1804.809858	62.504420	63.388071
1804.280281	59.131736	63.393076
1803.488318	59.158150	63.398081
1802.394100	54.906851	63.403086
1802.125423	51.025948	63.408090
1801.391396	61.358315	63.413095
1801.075379	58.621944	63.418100
1800.125961	48.009696	63.423105
1799.330256	55.612607	63.428110
1798.986233	45.970278	63.433114
1798.165468	54.699991	63.438119
1797.281948	49.833326	63.443124
1796.331551	52.608377	63.448129
1795.803358	51.559974	63.453134
1795.660325	54.709881	63.458138
1795.039734	58.118557	63.463143
1794.175549	56.465899	63.468148
1793.401952	57.479755	63.473153
1792.263630	58.956818	63.478158
1792.103251	57.164012	63.483162
1791.908920	55.595800	63.488167
1791.260727	49.007533	63.493172
1790.205267	45.510201	63.498177
1789.187561	56.024813	63.503182
1788.745904	51.942716	63.508186
1788.253878	54.223923	63.513191
1787.701217	52.192205	63.518196
1786.911104	50.176117	63.523201
1786.016400	55.489181	63.528206
1785.720482	56.704735	63.533210
1785.042018	50.428791	63.538215
1784.206259	46.393511	63.543220
1783.586224	58.403049	63.548225
1782.626684	54.556163	63.553230
1782.135334	46.476384	63.558234
1781.598684	49.576831	63.563239
1781.043455	51.473826	63.568244
1780.041745	54.712785	63.573249
1779.109078	52.654680	63.578254
1779.030977	48.008636	63.583258
1778.419777	47.288818	63.588263
1777.911492	54.273639	63.593268
1776.818123	50.277693	63.598273
1775.939195	48.644731	63.603278
1775.641436	52.680251	63.608282
1774.994945	56.113543	63.613287
1774.728227	49.343272	63.618292
1774.036610	51.834378	63.623297
1773.051105	56.822811	63.628302
1772.797696	51.127516	63.633306
1771.441170	59.958090	63.638311
1771.004412	61.025697	63.643316
1770.097091	51.879692	63.648321
1769.490972	50.387917	63.653326
1769.244491	47.943294	63.658330
1768.354111	59.360237	63.663335
1767.247563	53.584378	63.668340
1766.792776	50.138325	63.673345
1766.411007	57.215025	63.678350
1766.286444	55.530077	63.683354
1765.437873	59.831274	63.688359
1764.634291	51.555070	63.693364
1763.954490	45.582132	63.698369
1763.114875	53.819668	63.703374
1762.234197	51.840049	63.708378
1761.226554	61.768008	63.713383
1760.662674	55.033890	63.718388
1760.386365	49.722291	63.723393
1759.771241	63.185048	63.728398
1759.584990	52.563583	63.733402
1758.719619	57.398898	63.738407
1757.899207	50.325467	63.743412
1757.158699	49.582033	63.748417
1756.671559	53.365348	63.753422
1755.798007	50.640256	63.758426
1754.820243	57.825801	63.763431
1754.502851	54.206538	63.768436
1754.033589	45.902479	63.773441
1753.320065	56.756735	63.778446
1752.420958	44.699876	63.783450
1751.412793	53.647023	63.788455
1750.863628	54.025989	63.793460
1750.556432	49.957240	63.798465
1749.855184	52.853593	63.803470
1749.690589	45.655513	63.808474
1748.426291	53.695563	63.813479
1747.871802	55.289664	63.818484
1747.489260	49.250595	63.823489
1746.797026	57.242375	63.828494
1746.212522	51.247997	63.833498
1744.883111	48.719890	63.838503
1744.353716	51.025962	63.843508
1744.068213	49.076408	63.848513
1743.400237	55.930474	63.853518
1742.943531	51.134820	63.858522
1741.524133	58.243847	63.863527
1741.216663	44.006664	63.868532
1740.845607	47.440374	63.873537
1740.156317	56.639666	63.878542
1739.037013	41.173624	63.883546
1738.396908	48.915841	63.888551
1737.777482	52.179258	63.893556
1737.508598	51.917607	63.898561
1737.040501	50.673586	63.903566
1736.130922	41.527961	63.908570
1735.155225	53.273856	63.913575
1734.444346	45.900758	63.918580
1734.005618	47.000222	63.923585
1733.555426	55.481855	63.928590
1732.897035	53.504790	63.933594
1731.959689	50.256814	63.938599
1731.372244	53.180829	63.943604
1730.967571	45.776447	63.948609
1729.669552	57.706006	63.953614
1729.141014	55.052287	63.958618
1728.451701	51.883194	63.963623
1728.258054	48.785192	63.968628
1727.823400	45.613502	63.973633
1727.027889	47.277426	63.978638
1726.041762	46.825331	63.983642
1725.303614	55.239156	63.988647
1724.896618	50.755741	63.993652
1724.655262	50.652151	63.998657
1723.536049	59.580675	64.003662
1723.188378	48.251554	64.008666
1722.316605	53.127319	64.013671
1721.520163	58.746504	64.018676
1720.489700	50.610435	64.023681
1719.798916	55.351797	64.028686
1719.541337	48.001326	64.033690
1719.040596	47.610918	64.038695
1718.272195	50.100039	64.043700
1717.612717	48.003300	64.048705
1716.601242	56.712858	64.053710
1716.331663	49.449451	64.058714
1715.696352	50.078656	64.063719
1714.877268	50.104673	64.068724
1713.833924	48.447383	64.073729
1713.162867	57.058718	64.078734
1712.830097	48.786609	64.083738
1712.402566	54.246272	64.088743
1711.838105	51.180359	64.093748
1711.029194	60.171570	64.098753
1710.160739	53.265064	64.103758
1709.861422	44.881985	64.108762
1709.035565	50.849627	64.113767
1708.177725	52.846740	64.118772
1707.376703	53.661544	64.123777
1706.766685	52.235060	64.128782
1706.271788	46.802067	64.133786
1705.720587	56.143440	64.138791
1704.989208	44.469983	64.143796
1704.210399	48.485716	64.148801
1703.226659	50.893923	64.153806
1702.726146	47.123977	64.158810
1702.652569	49.420738	64.163815
1702.102471	59.608785	64.168820
1701.200055	45.562304	64.173825
1700.127298	47.421663	64.178830
1700.015640	49.992562	64.183834
1699.275443	44.232670	64.188839
1698.470090	49.187779	64.193844
1697.826967	48.040954	64.198849
1697.073792	50.101873	64.203854
1696.460375	50.145693	64.208858
1695.231220	56.825544	64.213863
1694.554404	51.822005	64.218868
1694.333077	45.790459	64.223873
1693.524005	52.051914	64.228878
1693.647902	47.271288	64.233882
1692.752791	53.447059	64.238887
1691.473091	45.629724	64.243892
1691.499226	44.162126	64.248897
1690.532108	60.215029	64.253902
1690.042793	42.666663	64.258906
1688.943635	45.331333	64.263911
1688.374535	45.689823	64.268916
1687.918652	44.905932	64.273921
1687.386929	47.310157	64.278926
1686.406256	40.252753	64.283930
1685.125191	53.936405	64.288935
1684.783051	49.349655	64.293940
1684.502458	45.759254	64.298945
1683.827916	41.130686	64.303950
1684.074843	38.420040	64.308954
1682.581466	49.893349	64.313959
1681.541028	49.804722	64.318964
1681.067567	45.729279	64.323969
1680.725935	48.502291	64.328974
1680.098702	40.250158	64.333978
1679.195807	47.111582	64.338983
1678.642601	44.666805	64.343988
1678.288854	43.336822	64.348993
1676.981912	44.534778	64.353998
1676.243351	41.469722	64.359002
1675.611939	43.323642	64.364007
1675.067487	41.990834	64.369012
1674.870983	41.459066	64.374017
1674.112464	49.926597	64.379022
1673.278076	46.037800	64.384026
1672.839107	45.910409	64.389031
1672.310504	43.046975	64.394036
1671.507810	39.831254	64.399041
1670.284724	45.127122	64.404046
1669.713163	51.822377	64.409050
1669.107321	58.661856	64.414055
1668.946150	55.782635	64.419060
1668.179453	46.732616	64.424065
1666.819872	56.681808	64.429070
1666.434577	46.404228	64.434074
1665.960578	50.084540	64.439079
1665.229761	54.717152	64.444084
1665.296484	46.039388	64.449089
1664.352949	54.708205	64.454094
1663.612874	42.802752	64.459098
1662.987981	47.968908	64.464103
1661.640666	50.015402	64.469108
1660.813235	48.800089	64.474113
1660.378439	49.897363	64.479118
1660.158256	46.581228	64.484122
1659.603520	54.678917	64.489127
1659.219703	45.312609	64.494132
1658.098444	51.240454	64.499137
1656.921250	45.832275	64.504142
1656.663248	48.656662	64.509146
1656.209713	47.588544	64.514151
1655.552778	55.174174	64.519156
1654.992643	49.636435	64.524161
1654.088255	51.510069	64.529166
1653.746862	48.400852	64.534170
1653.087105	47.174677	64.539175
1651.982600	57.742540	64.544180
1651.441970	51.378511	64.549185
1650.932601	50.691434	64.554190
1650.835920	51.842235	64.559194
1649.142779	46.397745	64.564199
1648.460525	47.466520	64.569204
1647.982232	44.637678	64.574209
1647.376901	50.217057	64.579214
1647.340550	51.064953	64.584218
1646.150015	44.163908	64.589223
1645.049868	43.841924	64.594228
1644.743712	47.277950	64.599233
1644.069118	54.243474	64.604238
1644.057010	39.574614	64.609242
1643.238222	48.502745	64.614247
1642.180503	48.197676	64.619252
1641.667018	43.813201	64.624257
1641.040037	59.149742	64.629262
1640.012967	44.252593	64.634266
1639.010479	50.773451	64.639271
1638.284682	55.493583	64.644276
1638.202575	52.669616	64.649281
1637.345661	53.277271	64.654286
1637.346120	52.014030	64.659290
1637.020969	69.280186	64.664295
1635.816231	53.457171	64.669300
1635.347585	52.921327	64.674305
1634.529529	55.200734	64.679310
1633.275887	54.857406	64.684314
1632.840381	49.668892	64.689319
1632.070438	55.189267	64.694324
1631.505677	48.690302	64.699329
1631.328380	56.581375	64.704334
1630.830909	47.956969	64.709338
1629.505179	49.574261	64.714343
1629.064744	53.119933	64.719348
1628.844881	55.007837	64.724353
1627.290195	55.420406	64.729358
1626.766918	49.731736	64.734362
1626.492612	52.385247	64.739367
1625.813755	55.956180	64.744372
1625.409629	45.057113	64.749377
1624.303604	50.137280	64.754382
1623.927786	43.146244	64.759386
1623.505447	49.868263	64.764391
1622.327141	52.813624	64.769396
1621.804292	47.752532	64.774401
1620.941799	53.218225	64.779406
1620.778336	50.774624	64.784410
1619.842175	47.461848	64.789415
1618.895622	54.287649	64.794420
1618.446935	46.054478	64.799425
1618.048784	58.576001	64.804430
1617.274758	49.814178	64.809434
1616.267061	50.116202	64.814439
1615.339960	53.707651	64.819444
1615.087430	40.243967	64.824449
1614.348438	53.286425	64.829454
1614.138256	43.659149	64.834458
1613.447578	49.632148	64.839463
1612.148683	45.768281	64.844468
1611.844482	43.227189	64.849473
1611.101719	53.898447	64.854478
1610.872872	48.853730	64.859482
1609.790714	45.389106	64.864487
1608.952768	54.320291	64.869492
1608.537664	44.531602	64.874497
1607.743897	49.540088	64.879502
1607.448479	44.934892	64.884506
1606.819674	57.019960	64.889511
1605.830409	52.586495	64.894516
1605.394323	50.899009	64.899521
1604.841763	58.510647	64.904526
1603.938825	43.070236	64.909530
1603.062613	52.016962	64.914535
1602.504422	52.578747	64.919540
1602.227702	45.858984	64.924545
1601.480498	49.611095	64.929550
1600.656720	44.632513	64.934554
1600.155530	52.411033	64.939559
1599.546715	46.106740	64.944564
1598.814470	42.808886	64.949569
1597.603910	49.394353	64.954574
1597.144417	45.160587	64.959578
1596.612129	50.173268	64.964583
1595.917609	48.996787	64.969588
1595.672010	42.549634	64.974593
1594.210697	52.978651	64.979598
1593.304718	48.484652	64.984602
1592.859982	53.100215	64.989607
1592.543234	53.415479	64.994612
1592.611963	46.017922	64.999617
1591.901413	52.940280	65.004622
1591.337607	42.739970	65.009626
1590.452905	50.943707	65.014631
1589.165531	54.887300	65.019636
1588.664694	50.339974	65.024641
1587.647553	56.524124	65.029646
1587.347621	53.830964	65.034650
1587.235315	50.029331	65.039655
1586.347479	53.665015	65.044660
1585.322690	45.264755	65.049665
1584.361306	53.699879	65.054670
1584.191413	44.220754	65.059674
1583.592346	42.584399	65.064679
1582.875350	59.964837	65.069684
1581.711764	42.982546	65.074689
1581.125041	56.962785	65.079694
1581.117037	52.307196	65.084698
1580.725393	53.250966	65.089703
1579.500986	51.732888	65.094708
1578.945755	46.077695	65.099713
1577.891297	54.022971	65.104718
1577.923158	50.709380	65.109722
1576.946125	46.756546	65.114727
1575.949939	52.498965	65.119732
1575.663179	51.090542	65.124737
1575.446342	51.635946	65.129742
1574.053657	46.954348	65.134746
1573.410117	50.401406	65.139751
1572.864623	48.114704	65.144756
1572.472244	45.841524	65.149761
1571.319314	57.744935	65.154766
1570.634786	52.215944	65.159770
1569.992991	51.169868	65.164775
1569.565970	50.879743	65.169780
1569.239435	44.898050	65.174785
1568.733696	50.378038	65.179790
1567.754022	50.521082	65.184794
1566.571723	47.734726	65.189799
1566.338328	52.808735	65.194804
1566.350113	48.728760	65.199809
1564.464968	56.949532	65.204814
1563.936143	51.908328	65.209818
1563.617939	57.645535	65.214823
1563.148062	63.074098	65.219828
1562.768087	55.142264	65.224833
1561.520725	56.209383	65.229838
1560.844571	61.760608	65.234842
1560.347600	60.860262	65.239847
1559.671229	59.266157	65.244852
1559.073154	50.670371	65.249857
1558.078882	63.677710	65.254862
1557.619692	53.564864	65.259866
1557.285795	49.424694	65.264871
1556.625698	47.514183	65.269876
1555.736656	46.403315	65.274881
1554.594252	60.020830	65.279886
1554.475623	56.485138	65.284890
1554.214338	57.077030	65.289895
1553.467728	52.822658	65.294900
1552.662358	55.916956	65.299905
1551.685753	57.811561	65.304910
1551.095737	53.891863	65.309914
1550.066661	55.488868	65.314919
1549.063751	59.229583	65.319924
1548.775815	49.707713	65.324929
1548.395433	59.911388	65.329934
1547.938328	44.193580	65.334938
1547.561561	50.793244	65.339943
1546.570020	57.911652	65.344948
1545.989275	49.954954	65.349953
1545.013194	57.983986	65.354958
1544.715426	57.760062	65.359962
1543.777586	52.755466	65.364967
1542.930174	51.043460	65.369972
1542.418625	51.747661	65.374977
1541.906744	61.688372	65.379982
1541.385073	48.429895	65.384986
1540.545235	48.981250	65.389991
1539.585762	46.243082	65.394996
1539.647054	51.323885	65.400001
1538.948026	54.901196	65.405006
1537.743917	50.604404	65.410010
1537.153249	49.630640	65.415015
1536.480280	58.634980	65.420020
1536.307949	54.809771	65.425025
1535.035465	59.998428	65.430030
1534.316146	54.448166	65.435034
1533.881804	56.061065	65.440039
1533.329221	61.002865	65.445044
1532.861285	50.546056	65.450049
1531.904190	58.624116	65.455054
1530.979074	71.253040	65.460058
1530.799359	58.050611	65.465063
1530.101225	66.573241	65.470068
1529.591659	56.861077	65.475073
1528.841644	62.326272	65.480078
1527.939155	59.405582	65.485082
1527.565954	59.433349	65.490087
1526.585676	63.411757	65.495092
1526.123464	53.045504	65.500097
1525.359758	58.706845	65.505102
1524.794989	54.106611	65.510106
1523.892738	48.993865	65.515111
1523.143466	52.131297	65.520116
1522.567711	54.837448	65.525121
1522.041985	56.559489	65.530126
1521.693038	60.387115	65.535130
1520.506535	49.584009	65.540135
1519.666619	54.178795	65.545140
1519.422364	55.871881	65.550145
1518.825959	58.094023	65.555150
1518.497259	48.712682	65.560154
1517.573402	56.446410	65.565159
1516.438940	62.852661	65.570164
1515.971356	54.441160	65.575169
1515.623925	63.475781	65.580174
1514.659162	59.653488	65.585178
1514.006571	61.007751	65.590183
1513.545403	68.447183	65.595188
1513.180688	56.922116	65.600193
1512.462688	60.762654	65.605198
1511.128030	63.846452	65.610202
1510.820752	61.307438	65.615207
1510.156330	59.418127	65.620212
1509.845581	51.543118	65.625217
1508.509648	55.349381	65.630222
1507.962235	56.346301	65.635226
1507.431077	52.666427	65.640231
1506.698162	59.824177	65.645236
1506.729676	52.651737	65.650241
1505.750387	61.580178	65.655246
1504.799535	59.848351	65.660250
1504.187097	59.026291	65.665255
1503.688969	62.671038	65.670260
1502.535781	60.214408	65.675265
1501.600726	50.163006	65.680270
1501.510778	59.341217	65.685274
1501.252590	50.399695	65.690279
1500.721151	50.299643	65.695284
1499.876924	51.003100	65.700289
1498.785112	52.217422	65.705294
1498.232341	53.284582	65.710298
1497.855156	46.377371	65.715303
1496.538644	55.834075	65.720308
1496.051960	39.685740	65.725313
1495.836690	43.648242	65.730318
1494.928607	47.026966	65.735322
1494.452039	44.855490	65.740327
1493.257150	48.350755	65.745332
1492.876248	50.835130	65.750337
1492.340765	46.312258	65.755342
1491.787533	49.363349	65.760346
1491.252086	46.661898	65.765351
1490.004458	49.698757	65.770356
1489.276913	50.101393	65.775361
1489.065999	53.713114	65.780366
1489.094369	40.078663	65.785370
1487.870128	38.874427	65.790375
1487.013780	43.099660	65.795380
1486.539845	40.096693	65.800385
1485.586144	45.990086	65.805390
1484.873568	41.198885	65.810394
1484.255189	42.030463	65.815399
1483.430628	50.481718	65.820404
1483.419051	43.147394	65.825409
1483.008193	51.170197	65.830414
1481.823172	45.466878	65.835418
1481.505403	42.715068	65.840423
1480.407319	45.540503	65.845428
1479.587829	48.835765	65.850433
1478.902618	49.372028	65.855438
1478.305727	35.135187	65.860442
1477.985056	42.400891	65.865447
1477.433668	45.856978	65.870452
1476.567053	39.557424	65.875457
1475.587748	51.937906	65.880462
1475.219124	45.239080	65.885466
1474.710093	46.234636	65.890471
1473.589982	43.250781	65.895476
1472.927399	41.329650	65.900481
1472.198434	45.886314	65.905486
1472.005925	39.720912	65.910490
1471.551843	31.641614	65.915495
1470.193445	42.606271	65.920500
1469.761008	37.262766	65.925505
1469.282759	47.737460	65.930510
1468.952904	42.773475	65.935514
1468.305805	44.223071	65.940519
1466.827030	48.791663	65.945524
1466.594454	47.882435	65.950529
1465.918028	53.897356	65.955534
1465.121824	48.209525	65.960538
1464.111780	48.702796	65.965543
1463.499432	55.488146	65.970548
1463.137716	37.746126	65.975553
1462.654435	50.270135	65.980558
1462.386526	41.210319	65.985562
1461.582355	28.305875	65.990567
1460.618799	40.658616	65.995572
1460.425048	37.645820	66.000577
1459.497060	44.104428	66.005582
1458.474333	48.917521	66.010586
1457.665648	40.393094	66.015591
1456.995325	55.921040	66.020596
1457.175305	41.267415	66.025601
1456.226753	51.495151	66.030606
1455.005987	47.320901	66.035610
1454.831327	42.813237	66.040615
1454.057574	46.823499	66.045620
1453.438798	42.227141	66.050625
1452.553780	43.468541	66.055630
1452.075989	42.118881	66.060634
1451.368740	47.580446	66.065639
1450.654712	48.988643	66.070644
1450.067228	39.996967	66.075649
1448.972842	42.571085	66.080654
1448.410707	50.017098	66.085658
1448.308206	47.106497	66.090663
1447.726067	40.624544	66.095668
1446.762216	51.072339	66.100673
1445.889815	45.721486	66.105678
1445.393484	46.950002	66.110682
1445.253192	42.105708	66.115687
1443.864245	47.391759	66.120692
1443.444841	47.348033	66.125697
1442.549615	47.949223	66.130702
1442.178543	44.466281	66.135706
1441.859681	30.420243	66.140711
1440.501117	50.783809	66.145716
1440.120143	40.504030	66.150721
1439.741616	40.849632	66.155726
1438.889045	45.395985	66.160730
1437.981285	40.109107	66.165735
1437.085481	45.376709	66.170740
1436.901207	34.285061	66.175745
1436.216160	38.621857	66.180750
1435.780281	37.404315	66.185754
1435.359985	37.501083	66.190759
1434.345436	43.270117	66.195764
1433.951572	36.969563	66.200769
1432.724108	46.971966	66.205774
1432.020108	42.671441	66.210778
1431.637669	41.500600	66.215783
1430.970934	49.904704	66.220788
1430.465418	37.089997	66.225793
1429.541656	44.292281	66.230798
1428.688094	48.562822	66.235802
1428.382054	40.680780	66.240807
1427.659329	46.715680	66.245812
1426.695739	43.888323	66.250817
1425.953973	42.028677	66.255822
1425.428265	42.392943	66.260826
1425.338061	37.072326	66.265831
1424.581582	50.040314	66.270836
1423.909221	40.850820	66.275841
1422.677344	47.701524	66.280846
1422.479738	48.740635	66.285850
1421.962029	40.740845	66.290855
1420.887709	46.880516	66.295860
1420.251514	40.236848	66.300865
1419.691682	43.741597	66.305870
1419.081687	40.394408	66.310874
1418.049212	41.725490	66.315879
1416.998889	47.060237	66.320884
1417.321913	37.384525	66.325889
1416.930021	40.627609	66.330894
1415.690006	49.308919	66.335898
1414.783246	44.599068	66.340903
1413.943230	45.300306	66.345908
1413.501694	40.921800	66.350913
1413.364161	45.650984	66.355918
1412.750396	49.303083	66.360922
1412.072136	45.400605	66.365927
1410.860242	52.651849	66.370932
1411.035966	39.380352	66.375937
1409.837690	50.308550	66.380942
1408.624767	44.198110	66.385946
1408.114428	48.779965	66.390951
1407.284660	49.586812	66.395956
1407.350158	45.712778	66.400961
1406.869079	51.444341	66.405966
1405.579255	51.628859	66.410970
1404.888212	45.344004	66.415975
1404.519348	45.517760	66.420980
1404.071213	43.083157	66.425985
1403.214154	46.031166	66.430990
1401.994659	58.061908	66.435994
1401.882742	45.173603	66.440999
1401.063626	54.811487	66.446004
1400.992169	46.029547	66.451009
1399.885214	50.152711	66.456014
1399.032043	49.115046	66.461018
1398.793958	43.016823	66.466023
1398.155929	43.039394	66.471028
1397.017933	45.640965	66.476033
1396.458577	44.824688	66.481038
1395.848098	46.724230	66.486042
1395.830387	39.356197	66.491047
1394.990376	40.841204	66.496052
1393.955301	33.294255	66.501057
1393.305722	50.227155	66.506062
1392.563965	51.109905	66.511066
1391.807622	34.233329	66.516071
1390.872624	51.362989	66.521076
1390.387405	40.404340	66.526081
1390.019661	42.675317	66.531086
1389.636108	45.854000	66.536090
1388.822412	42.403577	66.541095
1387.887746	45.978952	66.546100
1387.516281	39.572343	66.551105
1386.603204	44.084172	66.556110
1385.411879	52.262581	66.561114
1385.217084	41.645708	66.566119
1384.594612	40.612379	66.571124
1384.440758	41.461607	66.576129
1383.492904	42.640477	66.581134
1382.582123	40.597971	66.586138
1382.145161	34.419401	66.591143
1381.713841	45.854912	66.596148
1380.912795	30.778490	66.601153
1380.162433	39.814070	66.606158
1379.278396	39.011559	66.611162
1378.925432	33.256464	66.616167
1378.030296	44.300490	66.621172
1377.023695	44.247609	66.626177
1376.603264	35.469109	66.631182
1375.817703	39.949632	66.636186
1375.769829	40.920789	66.641191
1374.595784	46.719928	66.646196
1374.007182	39.280214	66.651201
1373.188849	42.990069	66.656206
1372.833504	40.867160	66.661210
1372.813771	42.795808	66.666215
1371.416898	41.229554	66.671220
1370.760793	41.423742	66.676225
1370.377753	48.262541	66.681230
1369.615154	39.801789	66.686234
1368.934719	42.619226	66.691239
1367.618107	54.020426	66.696244
1367.404407	40.325121	66.701249
1367.228136	43.406200	66.706254
1366.189386	52.944961	66.711258
1365.488593	43.663809	66.716263
1364.740631	49.183906	66.721268
1364.437962	38.896431	66.726273
1363.267690	42.234869	66.731278
1362.206486	46.606246	66.736282
1361.904038	44.088567	66.741287
1360.937634	48.067975	66.746292
1360.967447	37.825423	66.751297
1360.720738	40.532913	66.756302
1360.304980	32.843376	66.761306
1359.453011	30.345243	66.766311
1358.250963	38.301427	66.771316
1357.719191	40.134847	66.776321
1356.482876	35.269249	66.781326
1355.887449	40.153224	66.786330
1355.553226	30.376987	66.791335
1354.887288	44.335129	66.796340
1354.730797	34.283048	66.801345
1353.888516	52.651684	66.806350
1352.892948	41.121300	66.811354
1352.530454	36.206683	66.816359
1351.617158	38.275800	66.821364
1350.800792	44.182095	66.826369
1350.271930	39.781214	66.831374
1349.727312	39.951377	66.836378
1349.551095	39.247673	66.841383
1348.103325	45.404157	66.846388
1347.875618	43.637862	66.851393
1347.243976	49.273515	66.856398
1346.063485	55.855881	66.861402
1345.402346	48.287351	66.866407
1344.466642	58.226065	66.871412
1344.429810	53.690192	66.876417
1343.837641	54.334705	66.881422
1343.457006	50.167308	66.886426
1342.734616	45.138011	66.891431
1341.887620	47.094088	66.896436
1341.532489	38.538609	66.901441
1340.476706	49.884159	66.906446
1339.598216	55.372973	66.911450
1339.171121	46.276983	66.916455
1338.391843	53.379055	66.921460
1337.223703	50.699372	66.926465
1336.516535	46.935557	66.931470
1335.655058	47.853125	66.936474
1335.767574	44.916235	66.941479
1335.154946	51.711110	66.946484
1334.953037	51.981340	66.951489
1334.816905	50.963751	66.956494
1333.332573	51.105108	66.961498
1332.941953	47.789300	66.966503
1331.635434	56.851812	66.971508
1330.951419	54.784312	66.976513
1330.088048	57.376948	66.981518
1329.797915	63.697927	66.986522
1329.676816	59.211720	66.991527
1328.342796	56.444867	66.996532
1327.655498	54.395237	67.001537
1327.193357	52.382354	67.006542
1326.442723	52.916442	67.011546
1326.117965	47.584233	67.016551
1324.875496	51.214871	67.021556
1324.401307	50.661044	67.026561
1324.205414	52.423728	67.031566
1323.575272	52.210091	67.036570
1322.871312	44.933814	67.041575
1321.559336	61.782800	67.046580
1321.138448	47.723036	67.051585
1320.804760	44.734079	67.056590
1320.112450	57.180942	67.061594
1319.356263	48.753879	67.066599
1318.345559	53.680231	67.071604
1318.297949	51.789110	67.076609
1317.377874	55.746976	67.081614
1316.345213	48.515071	67.086618
1315.960728	55.273680	67.091623
1315.186970	52.337338	67.096628
1314.842508	47.639059	67.101633
1313.871055	49.170221	67.106638
1312.872672	49.803626	67.111642
1312.848681	51.348166	67.116647
1312.147312	53.301602	67.121652
1311.479441	51.195271	67.126657
1310.854769	47.758978	67.131662
1309.668892	54.242863	67.136666
1309.726297	43.268933	67.141671
1308.794999	50.620688	67.146676
1308.182919	53.646476	67.151681
1307.275187	53.940612	67.156686
1306.399104	57.959298	67.161690
1306.353902	46.823478	67.166695
1305.452691	55.931952	67.171700
1304.757953	51.005504	67.176705
1303.966176	56.788056	67.181710
1303.315141	60.977550	67.186714
1303.503600	45.647635	67.191719
1302.193438	45.699817	67.196724
1301.526415	49.226362	67.201729
1300.996167	45.336657	67.206734
1299.769975	51.404321	67.211738
1299.107250	42.834673	67.216743
1298.258024	43.584722	67.221748
1298.018254	48.390087	67.226753
1297.778284	47.896800	67.231758
1297.049470	57.933523	67.236762
1296.533276	47.714700	67.241767
1295.531553	48.615154	67.246772
1295.052657	46.004109	67.251777
1294.223597	48.603916	67.256782
1293.287275	51.271240	67.261786
1292.379274	50.251791	67.266791
1292.254556	55.032558	67.271796
1292.206164	53.095829	67.276801
1290.757487	56.529029	67.281806
1290.053345	55.379395	67.286810
1289.742551	49.557681	67.291815
1289.002325	50.183168	67.296820
1288.178196	48.477011	67.301825
1287.421781	46.878363	67.306830
1286.752237	44.371751	67.311834
1286.594170	46.161539	67.316839
1285.535216	55.457527	67.321844
1284.508049	49.592014	67.326849
1283.865077	51.657600	67.331854
1283.498358	49.057108	67.336858
1283.431851	50.297740	67.341863
1282.781152	51.006767	67.346868
1281.776743	44.921591	67.351873
1281.070547	48.195742	67.356878
1280.060590	49.289904	67.361882
1279.683860	43.201128	67.366887
1278.490872	50.894128	67.371892
1277.582866	38.200238	67.376897
1277.809724	51.152253	67.381902
1277.455292	50.497391	67.386906
1277.030729	40.341282	67.391911
1275.943447	49.100866	67.396916
1275.267832	50.272760	67.401921
1274.292550	43.700399	67.406926
1273.017896	57.575570	67.411930
1272.847088	52.554789	67.416935
1272.424026	58.193566	67.421940
1272.090274	41.784448	67.426945
1271.553753	51.923064	67.431950
1270.378593	54.491173	67.436954
1269.837858	49.242200	67.441959
1269.233395	48.450471	67.446964
1268.037581	47.489409	67.451969
1267.473163	46.399570	67.456974
1266.720466	51.160334	67.461978
1266.077307	48.031352	67.466983
1265.714621	48.101641	67.471988
1265.288982	37.764355	67.476993
1265.093332	41.769479	67.481998
1263.687173	54.012876	67.487002
1263.325164	40.620304	67.492007
1262.860103	49.574278	67.497012
1261.751706	49.417777	67.502017
1261.274995	49.271226	67.507022
1260.522175	49.290005	67.512026
1260.199205	52.681427	67.517031
1258.678055	57.517072	67.522036
1258.160255	51.190525	67.527041
1257.933222	49.244355	67.532046
1257.181599	63.033218	67.537050
1256.869951	50.526785	67.542055
1255.764280	59.379194	67.547060
1255.281189	46.527856	67.552065
1254.802268	51.006966	67.557070
1253.658669	52.011998	67.562074
1252.921989	40.705436	67.567079
1252.334549	48.453549	67.572084
1251.769805	48.574893	67.577089
1251.674702	42.763049	67.582094
1250.401355	56.830412	67.587098
1250.055605	53.080119	67.592103
1249.335857	54.727403	67.597108
1249.082173	51.492340	67.602113
1248.686921	45.592600	67.607118
1247.365974	52.796592	67.612122
1246.976775	43.331896	67.617127
1245.726354	45.126641	67.622132
1244.647789	44.151678	67.627137
1244.092083	43.692832	67.632142
1243.590778	51.655915	67.637146
1243.776874	42.282674	67.642151
1242.869063	50.166889	67.647156
1242.580723	46.569900	67.652161
1241.394424	43.356977	67.657166
1240.773345	50.501725	67.662170
1239.819284	42.626566	67.667175
1238.723432	45.513244	67.672180
1238.426758	42.113129	67.677185
1238.069661	42.534202	67.682190
1237.443512	50.539215	67.687194
1237.310596	39.191849	67.692199
1235.943691	47.749899	67.697204
1235.368788	54.652336	67.702209
1234.979873	42.941966	67.707214
1234.123344	48.495125	67.712218
1233.399140	45.815866	67.717223
1232.579839	51.594924	67.722228
1231.770005	51.126027	67.727233
1231.567306	44.728883	67.732238
1231.033258	49.483273	67.737242
1230.385457	43.055981	67.742247
1229.332625	48.066333	67.747252
1228.647907	52.789488	67.752257
1228.242241	48.446318	67.757262
1227.328524	43.654070	67.762266
1226.840714	43.701682	67.767271
1226.484539	47.746528	67.772276
1225.450643	44.640268	67.777281
1224.440710	41.941791	67.782286
1223.508269	45.026423	67.787290
1223.611035	46.776313	67.792295
1223.109457	41.574747	67.797300
1222.565609	45.674668	67.802305
1221.548543	41.994864	67.807310
1220.657787	50.382586	67.812314
1220.486539	45.503814	67.817319
1219.876907	43.530178	67.822324
1218.664696	51.248335	67.827329
1217.992615	48.724799	67.832334
1217.642452	51.781496	67.837338
1217.511844	46.921493	67.842343
1215.830134	48.750142	67.847348
1215.287949	49.126533	67.852353
1214.686504	54.068266	67.857358
1214.348569	55.407257	67.862362
1214.081896	45.199246	67.867367
1213.206370	42.400551	67.872372
1212.219878	55.952367	67.877377
1212.001823	46.115102	67.882382
1210.913064	41.691326	67.887386
1210.259829	44.260042	67.892391
1209.406266	46.789652	67.897396
1209.293713	46.933715	67.902401
1208.767058	46.213208	67.907406
1207.363139	51.549064	67.912410
1206.992228	34.452009	67.917415
1206.469733	50.457945	67.922420
1205.585887	55.361008	67.927425
1205.003061	47.704378	67.932430
1204.075378	45.018061	67.937434
1203.749561	44.207268	67.942439
1203.603591	51.446783	67.947444
1202.460618	51.508700	67.952449
1201.901829	44.775518	67.957454
1201.038137	48.420094	67.962458
1200.070873	42.918843	67.967463
1199.071747	49.004056	67.972468
1198.553141	46.098143	67.977473
1198.323861	43.348074	67.982478
1197.664123	57.101827	67.987482
1197.265914	45.328287	67.992487
1196.840173	51.634561	67.997492
1196.125454	48.557980	68.002497
1195.220987	57.435183	68.007502
1194.307398	54.639392	68.012506
1193.902847	53.732309	68.017511
1192.782470	55.752410	68.022516
1192.235879	48.634081	68.027521
1191.997161	55.224436	68.032526
1191.308840	52.618331	68.037530
1190.742178	47.307270	68.042535
1189.640131	58.289635	68.047540
1189.059945	57.929312	68.052545
1188.717411	41.450652	68.057550
1187.659749	49.893312	68.062554
1187.238042	43.909481	68.067559
1186.552125	45.783219	68.072564
1186.201908	44.686143	68.077569
1185.855025	46.624237	68.082574
1184.311206	42.856328	68.087578
1183.932061	42.683236	68.092583
1183.499689	41.681229	68.097588
1182.208702	42.971512	68.102593
1181.420919	47.468210	68.107598
1180.913052	49.535989	68.112602
1180.917231	42.016255	68.117607
1180.197100	41.665575	68.122612
1179.521549	37.213949	68.127617
1178.706683	37.988535	68.132622
1177.989607	46.086864	68.137626
1177.382305	42.728274	68.142631
1176.213647	42.846328	68.147636
1175.507387	38.929454	68.152641
1175.125466	37.400597	68.157646
1174.715741	43.172878	68.162650
1174.354804	43.436872	68.167655
1173.202678	40.311590	68.172660
1172.266113	41.449315	68.177665
1172.032189	33.984801	68.182670
1171.588998	45.078425	68.187674
1171.204050	40.066486	68.192679
1169.768787	37.487718	68.197684
1169.092278	43.269312	68.202689
1169.257969	42.281005	68.207694
1168.295242	46.404975	68.212698
1167.434925	40.894615	68.217703
1166.567629	39.747312	68.222708
1166.146665	43.930202	68.227713
1165.451022	42.038070	68.232718
1164.198207	50.417156	68.237722
1164.058167	38.780770	68.242727
1163.573539	44.288993	68.247732
1162.881824	45.170157	68.252737
1162.023987	42.792877	68.257742
1161.127017	45.614839	68.262746
1160.579090	35.732281	68.267751
1160.257432	44.319671	68.272756
1159.354171	43.630684	68.277761
1158.666521	34.653462	68.282766
1157.752451	42.895091	68.287770
1157.727941	33.449695	68.292775
1157.418636	43.228897	68.297780
1156.364489	39.236468	68.302785
1155.857217	44.270467	68.307790
1154.868670	48.478974	68.312794
1154.166456	36.107239	68.317799
1152.955908	39.048463	68.322804
1152.346190	50.706330	68.327809
1152.115302	35.583487	68.332814
1151.359999	46.463397	68.337818
1151.227158	37.620291	68.342823
1150.083421	46.322661	68.347828
1149.551391	48.484175	68.352833
1149.120824	38.690189	68.357838
1148.418204	33.817092	68.362842
1147.485951	45.458444	68.367847
1146.564233	36.794425	68.372852
1145.725897	43.571608	68.377857
1145.682416	46.085938	68.382862
1145.145029	45.819747	68.387866
1144.642657	41.001534	68.392871
1143.567234	44.520526	68.397876
1143.020313	43.789063	68.402881
1142.541432	43.183977	68.407886
1141.463375	45.743004	68.412890
1140.778933	38.257105	68.417895
1140.624427	42.981104	68.422900
1139.676299	44.555928	68.427905
1138.996203	40.445665	68.432910
1138.037582	47.987898	68.437914
1137.709865	35.365791	68.442919
1137.073720	36.179774	68.447924
1136.253306	40.136035	68.452929
1135.433467	39.496869	68.457934
1134.870577	43.735453	68.462938
1134.657555	41.380207	68.467943
1133.896212	45.387000	68.472948
1132.716184	45.248256	68.477953
1132.205773	41.487907	68.482958
1131.710175	37.668430	68.487962
1131.271401	40.392291	68.492967
1130.334031	32.602846	68.497972
1129.448445	44.591600	68.502977
1128.976900	44.754918	68.507982
1128.437383	42.216632	68.512986
1128.169809	34.869443	68.517991
1127.511404	35.904592	68.522996
1126.135684	45.121694	68.528001
1126.110851	33.689350	68.533006
1124.725844	47.052248	68.538010
1124.111358	38.762004	68.543015
1123.005611	48.052864	68.548020
1123.029432	36.262690	68.553025
1122.999263	27.942592	68.558030
1122.435299	41.342053	68.563034
1121.430945	42.501618	68.568039
1120.839669	42.584632	68.573044
1119.765801	37.182378	68.578049
1118.881213	38.434859	68.583054
1117.844622	41.851488	68.588058
1117.787548	34.511821	68.593063
1116.871303	38.987965	68.598068
1116.553113	38.738954	68.603073
1116.440198	37.056930	68.608078
1115.105914	35.875112	68.613082
1114.335926	32.624422	68.618087
1114.135953	38.521042	68.623092
1113.520037	39.306582	68.628097
1112.678246	43.534338	68.633102
1111.737593	44.013555	68.638106
1111.441395	36.569994	68.643111
1110.437656	43.755126	68.648116
1109.257844	35.505923	68.653121
1109.208864	35.800731	68.658126
1108.791971	40.910248	68.663130
1108.287771	42.168461	68.668135
1107.306733	38.612290	68.673140
1106.470338	40.314435	68.678145
1106.136562	38.230718	68.683150
1105.409293	49.273339	68.688154
1104.838552	46.940302	68.693159
1103.664029	48.153750	68.698164
1103.411141	44.735651	68.703169
1103.036626	46.578800	68.708174
1101.538868	50.854131	68.713178
1100.963562	44.893176	68.718183
1100.456739	34.007445	68.723188
1099.920664	49.419443	68.728193
1099.916934	47.046678	68.733198
1098.799909	48.847083	68.738202
1098.100639	43.632839	68.743207
1097.323760	47.235250	68.748212
1096.626987	41.976454	68.753217
1095.702918	41.733933	68.758222
1094.190247	47.590202	68.763226
1094.675989	38.282847	68.768231
1094.247349	37.015329	68.773236
1093.941059	36.838547	68.778241
1093.303212	32.450340	68.783246
1091.976484	41.907248	68.788250
1091.213474	41.330020	68.793255
1091.164669	46.962897	68.798260
1090.210910	38.305577	68.803265
1089.712820	32.893754	68.808270
1088.829127	46.128034	68.813274
1088.349071	40.125124	68.818279
1087.354165	45.362860	68.823284
1086.388037	49.892684	68.828289
1086.283330	38.296426	68.833294
1085.762662	47.847474	68.838298
1085.009901	36.142989	68.843303
1084.043316	35.173938	68.848308
1083.803157	33.654086	68.853313
1082.760598	34.695160	68.858318
1081.622360	37.768418	68.863322
1081.011473	39.851024	68.868327
1080.688014	43.357657	68.873332
1080.034705	35.141416	68.878337
1079.901054	36.332804	68.883342
1079.105203	39.622840	68.888346
1078.317983	40.408829	68.893351
1077.672803	42.887983	68.898356
1077.232001	43.346048	68.903361
1076.131027	37.880316	68.908366
1074.915849	46.365414	68.913370
1075.083979	38.406440	68.918375
1074.435162	38.962251	68.923380
1073.568204	36.928662	68.928385
1072.769618	33.229940	68.933390
1072.308685	46.811720	68.938394
1071.562897	38.946089	68.943399
1071.203055	48.515711	68.948404
1070.247757	41.774681	68.953409
1069.675875	40.764925	68.958414
1068.652549	46.382510	68.963418
1068.060078	38.047782	68.968423
1068.033928	36.709934	68.973428
1066.990449	41.807165	68.978433
1066.458218	36.668865	68.983438
1066.218002	46.467043	68.988442
1065.351969	46.216878	68.993447
1064.321284	43.144872	68.998452
1063.437455	45.639915	69.003457
1063.105362	38.053837	69.008462
1061.952213	44.075283	69.013466
1061.369773	44.199484	69.018471
1061.246334	44.236473	69.023476
1060.477759	51.101934	69.028481
1060.030378	42.966479	69.033486
1058.547074	44.676932	69.038490
1058.087868	37.691407	69.043495
1057.585852	36.536496	69.048500
1057.230146	38.651053	69.053505
1056.985644	35.703147	69.058510
1055.848499	46.136029	69.063514
1055.124701	37.396410	69.068519
1054.651646	45.818651	69.073524
1053.582889	45.247495	69.078529
1053.054553	38.635675	69.083534
1052.249050	43.731325	69.088538
1052.171529	41.316684	69.093543
1051.270239	42.422032	69.098548
1050.020003	40.969829	69.103553
1049.561920	35.431800	69.108558
1048.858625	41.657657	69.113562
1048.756507	40.476977	69.118567
1048.095418	35.576806	69.123572
1046.760385	39.619691	69.128577
1046.428510	28.035932	69.133582
1045.872190	45.846586	69.138586
1045.530123	34.174556	69.143591
1044.492736	39.614608	69.148596
1043.950071	39.232581	69.153601
1043.643226	38.820923	69.158606
1042.547163	38.741405	69.163610
1041.441339	39.174383	69.168615
1041.010188	36.986316	69.173620
1040.445947	35.764036	69.178625
1040.219421	32.341755	69.183630
1039.452117	43.045392	69.188634
1038.505062	42.163140	69.193639
1038.131025	38.573510	69.198644
1037.131905	34.577114	69.203649
1036.416709	35.320118	69.208654
1035.390289	46.612195	69.213658
1034.916656	45.446464	69.218663
1035.051124	33.745934	69.223668
1034.375608	49.560171	69.228673
1034.055750	39.696563	69.233678
1033.103404	51.235484	69.238682
1032.229076	44.601439	69.243687
1031.041254	47.625837	69.248692
1030.217785	47.826238	69.253697
1030.118915	40.501112	69.258702
1029.777848	44.769081	69.263706
1028.621078	34.945582	69.268711
1028.277169	34.828410	69.273716
1027.403517	41.505583	69.278721
1026.848019	38.922555	69.283726
1025.414158	38.939365	69.288730
1025.210628	36.745050	69.293735
1024.683808	35.453741	69.298740
1024.200548	40.852951	69.303745
1023.497656	41.070442	69.308750
1022.483007	49.578853	69.313754
1022.496102	47.189220	69.318759
1021.654722	43.541478	69.323764
1020.666564	47.343108	69.328769
1020.189655	41.897966	69.333774
1018.958921	46.107203	69.338778
1018.677650	39.955989	69.343783
1018.275505	38.654307	69.348788
1017.283859	45.913240	69.353793
1016.645816	44.836751	69.358798
1016.103645	46.353340	69.363802
1015.659237	40.764255	69.368807
1015.301902	42.401250	69.373812
1014.313088	46.642964	69.378817
1014.090851	36.166154	69.383822
1012.600243	44.709288	69.388826
1011.442298	41.851521	69.393831
1010.803282	43.531756	69.398836
1011.110025	54.662202	69.403841
1010.628166	35.646326	69.408846
1009.859785	42.013436	69.413850
1008.966578	40.600646	69.418855
1008.330962	41.495003	69.423860
1007.270554	50.550027	69.428865
1006.988359	49.562006	69.433870
1005.803364	42.412840	69.438874
1005.457733	43.746771	69.443879
1005.096497	37.046876	69.448884
1004.412297	50.083854	69.453889
1004.103298	37.537653	69.458894
1003.197254	47.555308	69.463898
1002.354765	37.689704	69.468903
1001.389035	38.150873	69.473908
1000.224743	46.914915	69.478913
999.587513	39.132965	69.483918
999.112908	47.077632	69.488922
998.600878	37.813900	69.493927
998.699639	42.275248	69.498932
998.094765	45.730468	69.503937
997.374575	40.055954	69.508942
996.013208	48.083362	69.513946
995.614907	36.708879	69.518951
995.315257	35.493397	69.523956
994.014300	38.977365	69.528961
993.423223	33.361161	69.533966
992.592763	35.792540	69.538970
992.735128	35.672122	69.543975
992.196276	32.920872	69.548980
990.726835	45.149212	69.553985
990.439650	41.832782	69.558990
989.757567	48.044241	69.563994
988.844950	44.557658	69.568999
988.223126	38.358131	69.574004
987.295860	46.524635	69.579009
987.392524	37.381681	69.584014
986.841459	41.366092	69.589018
985.527339	40.690500	69.594023
985.031617	32.258405	69.599028
984.433784	43.146403	69.604033
984.146926	32.523763	69.609038
982.978658	37.590414	69.614042
982.111670	33.353818	69.619047
981.625235	34.468876	69.624052
981.078206	42.309946	69.629057
980.688301	33.805820	69.634062
979.756148	36.411082	69.639066
979.244392	31.187547	69.644071
978.774639	34.988705	69.649076
977.826889	51.928076	69.654081
977.246660	37.431730	69.659086
976.390589	38.446328	69.664090
976.107088	40.773338	69.669095
975.311006	31.639970	69.674100
974.300230	40.395360	69.679105
973.759245	40.364749	69.684110
973.276208	31.407081	69.689114
972.627761	47.018313	69.694119
971.565352	43.987666	69.699124
971.081494	42.495563	69.704129
970.718057	36.781641	69.709134
970.053404	34.737977	69.714138
969.258342	40.879103	69.719143
968.329868	31.192782	69.724148
967.594678	42.268221	69.729153
967.478699	35.475693	69.734158
966.599786	34.551087	69.739162
965.888671	35.865905	69.744167
965.286895	32.978014	69.749172
964.291881	46.528083	69.754177
964.159798	39.299714	69.759182
963.321378	47.844757	69.764186
962.553521	44.494426	69.769191
961.974805	37.117927	69.774196
961.582780	48.674941	69.779201
960.953146	43.315618	69.784206
959.490758	38.519322	69.789210
959.071381	41.851991	69.794215
958.715673	44.346613	69.799220
958.250690	51.580113	69.804225
957.599520	40.375187	69.809230
956.679670	41.336861	69.814234
956.037050	43.266845	69.819239
955.620132	34.817487	69.824244
954.510158	46.302657	69.829249
953.825703	37.742901	69.834254
953.490095	45.816844	69.839258
952.896234	41.574644	69.844263
951.966892	35.853002	69.849268
950.959480	40.387860	69.854273
950.747322	33.424556	69.859278
950.217984	35.133084	69.864282
949.840761	37.971758	69.869287
948.938062	38.481265	69.874292
948.031055	44.286967	69.879297
947.633053	37.015759	69.884302
946.678533	40.313733	69.889306
945.445368	46.699626	69.894311
945.381540	40.395549	69.899316
944.668601	45.257297	69.904321
944.362376	36.164265	69.909326
943.958666	36.938154	69.914330
942.705637	39.928809	69.919335
942.536758	39.433707	69.924340
941.400004	41.980076	69.929345
940.480651	47.939136	69.934350
939.574736	36.028844	69.939354
939.475830	37.552183	69.944359
939.400577	39.871289	69.949364
938.432123	40.772894	69.954369
937.340861	31.561933	69.959374
936.657174	35.006050	69.964378
936.115804	31.432030	69.969383
935.937322	28.114083	69.974388
934.999659	37.655801	69.979393
934.293637	33.981824	69.984398
933.618333	35.920167	69.989402
932.707558	35.789134	69.994407
931.895714	31.047034	69.999412
931.388934	37.176986	70.004417
931.269124	33.753507	70.009422
930.613911	41.282209	70.014426
929.860525	40.492184	70.019431
929.128629	45.017902	70.024436
927.986136	44.007517	70.029441
927.695900	34.957677	70.034446
926.861225	36.296899	70.039450
925.740722	34.899810	70.044455
925.496327	34.624888	70.049460
924.528196	40.148580	70.054465
924.704376	32.765507	70.059470
923.721963	40.071884	70.064474
922.904399	38.490968	70.069479
922.415030	37.534350	70.074484
921.754117	43.829185	70.079489
921.494145	33.020927	70.084494
920.349123	46.492374	70.089498
919.572461	42.563130	70.094503
919.336354	40.919646	70.099508
918.198432	49.867184	70.104513
917.422916	36.151007	70.109518
916.641548	33.168705	70.114522
915.907004	40.569682	70.119527
915.889595	39.068018	70.124532
915.425463	40.882873	70.129537
914.506624	41.973714	70.134542
913.906475	45.648976	70.139546
913.269983	39.213682	70.144551
912.699096	37.047878	70.149556
911.561381	48.867067	70.154561
911.204015	34.813110	70.159566
910.528082	42.218954	70.164570
909.675789	38.748037	70.169575
909.077828	38.519922	70.174580
908.147908	40.325324	70.179585
907.832893	34.742484	70.184590
907.463188	35.673396	70.189594
906.206831	42.960296	70.194599
905.469442	47.926872	70.199604
904.927853	46.730981	70.204609
904.552863	34.576940	70.209614
904.273800	39.710275	70.214618
903.327754	45.514318	70.219623
902.623023	40.747295	70.224628
902.012926	45.296214	70.229633
901.083015	33.503305	70.234638
900.309141	34.823397	70.239642
899.644217	38.043760	70.244647
899.311673	36.704214	70.249652
898.839555	39.528033	70.254657
897.846208	33.882834	70.259662
896.794189	45.145906	70.264666
896.172721	39.031508	70.269671
895.911394	37.177571	70.274676
895.815074	39.175172	70.279681
894.892038	38.131454	70.284686
894.058707	40.213231	70.289690
893.291850	41.513285	70.294695
892.950203	35.368550	70.299700
891.541271	44.381301	70.304705
891.402097	41.798282	70.309710
890.565517	40.144708	70.314714
889.957397	38.054222	70.319719
889.107257	32.753673	70.324724
888.194418	41.154453	70.329729
888.064136	38.136349	70.334734
887.614787	40.035590	70.339738
886.760293	43.215163	70.344743
886.028194	45.287140	70.349748
885.378820	45.529268	70.354753
884.923524	42.178107	70.359758
884.419365	37.144199	70.364762
883.184585	44.325172	70.369767
882.494175	41.598068	70.374772
882.203950	45.091545	70.379777
881.625751	30.613844	70.384782
880.602714	39.107858	70.389786
879.777390	44.703457	70.394791
879.600696	36.925526	70.399796
878.842715	41.652529	70.404801
878.207170	42.714065	70.409806
877.521660	38.806601	70.414810
876.625445	45.096316	70.419815
876.212545	38.989731	70.424820
875.117074	46.208462	70.429825
874.725215	42.981250	70.434830
874.302912	48.648330	70.439834
873.566000	45.698388	70.444839
873.011236	51.621522	70.449844
871.835594	46.923146	70.454849
871.112879	37.377589	70.459854
870.730563	46.394119	70.464858
870.319745	52.053065	70.469863
869.396268	39.524269	70.474868
868.564376	47.722936	70.479873
868.291671	38.365959	70.484878
867.821988	43.863956	70.489882
867.085865	37.289991	70.494887
866.450491	38.794634	70.499892
865.586399	42.440950	70.504897
864.906880	38.858971	70.509902
863.840257	43.456902	70.514906
862.828593	47.948315	70.519911
862.821137	46.270022	70.524916
862.283739	45.182285	70.529921
861.983818	41.088874	70.534926
860.866122	39.954724	70.539930
859.954097	44.917565	70.544935
859.351199	43.805560	70.549940
858.867998	46.251099	70.554945
858.732914	43.106026	70.559950
857.738199	38.727378	70.564954
856.516225	44.857631	70.569959
856.626355	43.105429	70.574964
855.765148	46.815946	70.579969
854.777211	40.886047	70.584974
853.946532	43.035224	70.589978
853.635200	45.712033	70.594983
853.425269	39.946893	70.599988
852.226427	46.451942	70.604993
851.492465	36.729984	70.609998
850.902794	50.999328	70.615002
850.479052	47.785079	70.620007
850.320928	39.231476	70.625012
848.522844	46.585701	70.630017
848.224954	39.461011	70.635022
847.945398	46.750163	70.640026
847.258886	50.792430	70.645031
846.299755	35.435489	70.650036
845.411159	50.339047	70.655041
844.975854	39.232274	70.660046
844.817624	38.913683	70.665050
843.755881	48.139284	70.670055
843.244855	40.088137	70.675060
842.444835	46.144928	70.680065
842.142735	42.936553	70.685070
841.143549	35.586015	70.690074
840.563274	46.851290	70.695079
840.187937	38.594041	70.700084
838.748783	51.393231	70.705089
837.911854	39.580818	70.710094
837.886747	44.175411	70.715098
837.066884	41.256033	70.720103
836.750675	41.451452	70.725108
835.598667	43.598163	70.730113
834.719588	35.498369	70.735118
834.326857	48.656134	70.740122
833.965937	44.637091	70.745127
833.619110	34.777826	70.750132
832.328947	42.797126	70.755137
831.912454	33.650707	70.760142
831.399729	41.268712	70.765146
830.576007	47.977418	70.770151
829.968188	39.624709	70.775156
829.011230	43.490825	70.780161
828.347871	36.788595	70.785166
828.108870	31.081707	70.790170
826.945291	36.600269	70.795175
826.246161	37.583627	70.800180
825.559262	51.057881	70.805185
825.203590	39.123139	70.810190
824.918133	43.634590	70.815194
824.099984	41.957605	70.820199
823.133339	35.748361	70.825204
822.637357	42.240893	70.830209
822.487094	31.131339	70.835214
821.417807	34.674708	70.840218
820.136633	39.790938	70.845223
820.446548	31.197537	70.850228
819.188170	42.111848	70.855233
818.437934	37.462486	70.860238
817.667861	36.820234	70.865242
817.352161	36.931995	70.870247
816.806430	36.947904	70.875252
816.201479	48.534084	70.880257
815.238393	36.396407	70.885262
814.647669	42.564970	70.890266
813.953407	39.988313	70.895271
813.758034	37.070466	70.900276
812.479376	39.723057	70.905281
811.682889	39.452448	70.910286
811.489297	35.081919	70.915290
810.843584	46.433308	70.920295
810.288798	40.978539	70.925300
808.856199	41.211317	70.930305
808.529048	42.575447	70.935310
808.329860	41.107451	70.940314
807.227828	50.388365	70.945319
806.931447	43.594607	70.950324
805.439908	45.722838	70.955329
805.383710	51.530348	70.960334
805.185968	42.916823	70.965338
804.212222	41.464889	70.970343
803.447967	47.634271	70.975348
802.738344	47.947513	70.980353
802.718945	50.103186	70.985358
801.359661	41.094231	70.990362
800.550337	46.103822	70.995367
800.344867	41.766723	71.000372
799.667764	52.375626	71.005377
798.753083	42.742378	71.010382
798.210279	45.258917	71.015386
797.208489	50.396920	71.020391
797.012458	42.309836	71.025396
796.106966	49.171920	71.030401
795.433414	37.063857	71.035406
795.051254	36.850303	71.040410
794.488433	49.249809	71.045415
793.756842	46.324279	71.050420
792.614764	42.027464	71.055425
792.195273	38.847246	71.060430
791.817854	45.727771	71.065434
790.773555	40.917067	71.070439
790.022961	41.385071	71.075444
789.214480	40.256924	71.080449
788.697134	47.049336	71.085454
788.669392	43.243774	71.090458
787.939943	50.763823	71.095463
787.127307	42.924709	71.100468
786.394829	53.805787	71.105473
785.655102	45.286427	71.110478
784.584939	50.585132	71.115482
784.182259	48.017260	71.120487
783.571071	44.459121	71.125492
783.166395	49.262373	71.130497
782.280564	41.354489	71.135502
781.569876	39.103738	71.140506
780.668355	48.784833	71.145511
780.434602	40.211739	71.150516
780.137987	47.505187	71.155521
779.294183	52.230110	71.160526
778.203432	41.044767	71.165530
777.278463	39.772739	71.170535
777.320112	43.702256	71.175540
776.409416	43.139175	71.180545
775.617821	37.009320	71.185550
774.946551	39.582583	71.190554
774.741288	48.012683	71.195559
774.009064	45.584009	71.200564
772.836975	46.076539	71.205569
772.464344	46.402376	71.210574
771.973032	49.812755	71.215578
770.606899	42.336158	71.220583
769.943194	38.444180	71.225588
769.488039	44.135423	71.230593
769.249603	43.927378	71.235598
768.868776	31.261789	71.240602
767.536378	44.651145	71.245607
767.115895	35.027553	71.250612
766.693015	48.880835	71.255617
766.073631	42.975883	71.260622
765.273740	35.864895	71.265626
764.281510	38.038241	71.270631
763.963456	33.838923	71.275636
763.368546	40.478100	71.280641
762.101849	38.732193	71.285646
761.248797	35.311917	71.290650
760.543471	42.463845	71.295655
760.417883	34.379749	71.300660
760.424824	45.620934	71.305665
759.679717	40.503989	71.310670
758.945305	43.371166	71.315674
758.073435	49.272258	71.320679
757.230295	34.592349	71.325684
756.147480	35.829200	71.330689
755.322348	34.806220	71.335694
755.340044	40.914202	71.340698
754.905604	49.393404	71.345703
754.229558	39.512449	71.350708
753.001825	43.961026	71.355713
752.587145	38.633781	71.360718
752.365014	36.087637	71.365722
751.048627	42.818024	71.370727
750.574318	36.700745	71.375732
749.732812	41.936248	71.380737
749.467610	38.313577	71.385742
748.855095	33.897785	71.390746
747.487981	37.554831	71.395751
747.096199	35.379478	71.400756
746.361112	36.890563	71.405761
746.275947	37.642154	71.410766
745.719818	39.577340	71.415770
744.457487	49.440469	71.420775
743.949145	44.702156	71.425780
743.792323	39.325976	71.430785
742.728667	43.932942	71.435790
742.288444	40.155206	71.440794
741.378152	44.288316	71.445799
740.620235	45.096551	71.450804
739.487084	45.918794	71.455809
738.933902	40.949499	71.460814
738.406274	53.064284	71.465818
737.837737	52.147116	71.470823
737.837403	44.030461	71.475828
737.226657	50.653244	71.480833
736.058930	43.148234	71.485838
735.517355	34.251994	71.490842
734.778933	36.569448	71.495847
734.014374	36.956112	71.500852
732.774083	40.246040	71.505857
732.928915	36.332566	71.510862
732.461164	38.351457	71.515866
731.481849	45.491820	71.520871
730.785050	30.031680	71.525876
730.000157	43.283417	71.530881
729.628045	41.138051	71.535886
729.503850	37.186998	71.540890
727.977456	40.691216	71.545895
727.454159	38.246641	71.550900
727.152464	42.246589	71.555905
726.102051	38.140223	71.560910
725.200267	30.783698	71.565914
724.228294	39.895690	71.570919
724.477569	33.593828	71.575924
723.991578	36.016177	71.580929
722.680925	33.227022	71.585934
722.099895	37.079052	71.590938
721.451626	35.569024	71.595943
721.282135	35.788407	71.600948
720.134734	39.224402	71.605953
719.276312	38.755523	71.610958
718.910290	31.764714	71.615962
718.435316	39.222178	71.620967
717.951117	45.780658	71.625972
716.296700	37.651395	71.630977
715.795983	37.015176	71.635982
715.754093	32.973749	71.640986
715.002714	38.966054	71.645991
714.647402	44.280278	71.650996
713.770755	38.622889	71.656001
713.160438	40.415320	71.661006
712.643469	34.047797	71.666010
711.353973	43.374357	71.671015
710.639303	33.453841	71.676020
710.192827	34.964715	71.681025
709.694511	35.062986	71.686030
709.502545	35.886777	71.691034
708.096361	38.583377	71.696039
707.722676	27.753852	71.701044
707.167820	39.770460	71.706049
706.114495	41.546695	71.711054
705.242670	38.583599	71.716058
704.765546	34.491621	71.721063
704.740856	31.668037	71.726068
703.962514	34.595838	71.731073
702.901642	36.067342	71.736078
701.901168	41.492176	71.741082
701.550731	42.569861	71.746087
701.284058	35.738281	71.751092
700.759508	34.106055	71.756097
699.798332	30.835486	71.761102
699.284611	33.257522	71.766106
698.318390	41.985402	71.771111
698.319556	29.738414	71.776116
697.334356	29.423772	71.781121
696.581908	37.187196	71.786126
695.771827	35.589396	71.791130
694.486979	39.971397	71.796135
694.051575	37.181670	71.801140
693.565455	38.722514	71.806145
693.058209	39.426193	71.811150
692.893934	33.035634	71.816154
691.796926	37.327802	71.821159
691.175787	34.591304	71.826164
690.315123	34.692081	71.831169
689.566297	33.305307	71.836174
689.618020	35.563194	71.841178
688.444823	42.535741	71.846183
687.818846	35.997921	71.851188
687.077524	37.514745	71.856193
686.686727	31.628619	71.861198
686.037557	35.453658	71.866202
685.059531	39.897196	71.871207
684.608080	24.281320	71.876212
683.994546	31.144248	71.881217
683.114759	34.878273	71.886222
682.496651	39.384353	71.891226
681.819989	43.991222	71.896231
681.541544	33.364158	71.901236
680.763933	36.619860	71.906241
679.583735	41.918776	71.911246
678.975699	28.090892	71.916250
678.358131	47.299047	71.921255
678.393201	27.064003	71.926260
677.532282	39.446321	71.931265
676.239074	38.158851	71.936270
676.147173	31.829311	71.941274
675.603804	37.167173	71.946279
674.793932	37.299292	71.951284
673.855554	37.562262	71.956289
673.368608	39.221515	71.961294
673.037566	30.233424	71.966298
671.409728	40.899111	71.971303
671.153926	36.896479	71.976308
670.359973	38.975208	71.981313
669.813387	40.544609	71.986318
669.869084	33.671164	71.991322
669.136072	36.997040	71.996327
668.115834	31.837208	72.001332
667.373145	37.446511	72.006337
666.642697	35.667304	72.011342
665.909442	26.374253	72.016346
665.004082	34.948942	72.021351
664.704975	32.752539	72.026356
664.410380	32.397327	72.031361
663.934366	39.232055	72.036366
662.905189	26.606665	72.041370
662.011115	39.178772	72.046375
661.700025	35.320566	72.051380
660.780728	34.071336	72.056385
659.934464	32.469849	72.061390
659.176745	29.316711	72.066394
658.971472	38.634643	72.071399
658.509307	31.329570	72.076404
657.323389	36.288776	72.081409
656.584906	35.611583	72.086414
656.834044	31.194229	72.091418
655.198649	39.349003	72.096423
654.788824	32.070289	72.101428
654.142279	30.285611	72.106433
653.357906	33.487203	72.111438
653.336470	30.704105	72.116442
652.126377	37.042287	72.121447
651.474915	33.433831	72.126452
651.180624	38.235285	72.131457
649.960954	38.666062	72.136462
649.492350	38.685496	72.141466
648.671600	40.043090	72.146471
648.290944	36.306352	72.151476
647.626639	32.356161	72.156481
646.879611	40.369473	72.161486
646.137745	38.087459	72.166490
645.410515	37.179814	72.171495
645.028657	30.940609	72.176500
644.486335	42.310245	72.181505
643.059324	37.913801	72.186510
643.041716	31.192383	72.191514
642.293923	39.781413	72.196519
641.917980	31.409193	72.201524
640.966956	38.160293	72.206529
640.158705	39.241505	72.211534
639.701121	35.006080	72.216538
639.113641	31.810068	72.221543
638.388328	26.194849	72.226548
637.470468	34.154938	72.231553
636.726774	32.242231	72.236558
636.673148	28.056021	72.241562
635.344940	33.296519	72.246567
634.879957	31.001955	72.251572
634.183508	31.250068	72.256577
633.559503	30.772273	72.261582
633.671618	30.084210	72.266586
632.460797	36.547097	72.271591
631.895113	30.110084	72.276596
631.424512	33.247521	72.281601
629.980853	36.934164	72.286606
629.360717	26.907165	72.291610
628.452207	31.322303	72.296615
628.037973	28.988119	72.301620
627.648849	26.397621	72.306625
627.512109	29.205919	72.311630
627.091509	19.793709	72.316634
626.324151	32.139055	72.321639
625.350175	30.464877	72.326644
624.069800	33.396956	72.331649
623.260389	28.332883	72.336654
622.737324	28.618042	72.341658
622.384722	38.235407	72.346663
622.282314	29.299229	72.351668
621.442721	29.716800	72.356673
620.343129	30.729296	72.361678
619.996274	26.692289	72.366682
619.474012	38.787293	72.371687
618.385065	31.127880	72.376692
617.697156	40.241974	72.381697
617.216107	40.700218	72.386702
616.758118	29.761138	72.391706
615.732705	35.508519	72.396711
615.040632	36.085528	72.401716
614.612694	39.709768	72.406721
614.285944	38.681583	72.411726
613.552745	26.012237	72.416730
612.161213	39.578225	72.421735
611.745434	35.323533	72.426740
611.649232	29.384199	72.431745
610.425118	43.891792	72.436750
609.820736	25.613128	72.441754
609.218347	37.148451	72.446759
608.676083	37.491865	72.451764
608.564664	26.738872	72.456769
607.076460	35.103622	72.461774
606.433412	27.740638	72.466778
605.558462	37.280341	72.471783
605.710046	31.262121	72.476788
604.588679	28.293074	72.481793
603.581801	37.063724	72.486798
603.460194	34.941565	72.491802
602.613686	39.816777	72.496807
602.033951	30.701152	72.501812
601.109971	35.911982	72.506817
600.218188	40.039035	72.511822
600.178671	34.317758	72.516826
599.566448	32.325776	72.521831
598.771190	33.289812	72.526836
598.187566	33.806974	72.531841
597.319558	36.004753	72.536846
597.012542	34.867770	72.541850
595.996367	36.131923	72.546855
595.484495	27.046495	72.551860
594.689452	27.100583	72.556865
594.101674	25.886890	72.561870
593.509522	31.923247	72.566874
592.389902	34.509613	72.571879
592.173434	32.448294	72.576884
591.536015	27.811010	72.581889
590.478410	31.213833	72.586894
589.973792	19.840642	72.591898
589.283075	39.615536	72.596903
588.914381	34.725712	72.601908
588.503044	28.801879	72.606913
587.786211	36.755198	72.611918
586.929148	36.711932	72.616922
586.173706	30.718323	72.621927
585.242774	34.238171	72.626932
584.456165	32.130463	72.631937
583.861225	31.925599	72.636942
584.075765	24.616851	72.641946
582.978911	37.413661	72.646951
582.076313	28.379429	72.651956
581.307442	27.292354	72.656961
580.639946	29.287888	72.661966
580.496043	23.203192	72.666970
579.379691	24.093793	72.671975
578.665152	27.405709	72.676980
578.142704	23.915503	72.681985
577.378304	39.617770	72.686990
577.458701	20.039444	72.691994
576.009877	26.215401	72.696999
575.290278	28.548823	72.702004
574.934829	24.084257	72.707009
574.567732	28.599261	72.712014
573.674192	30.075706	72.717018
572.575831	27.941961	72.722023
572.486498	25.880897	72.727028
571.965260	26.785527	72.732033
570.878324	35.846485	72.737038
570.075443	31.273407	72.742042
569.297718	41.844748	72.747047
569.205735	38.847381	72.752052
568.390023	32.677294	72.757057
567.292734	29.601927	72.762062
566.626296	28.239918	72.767066
566.155468	30.200977	72.772071
565.979848	28.850680	72.777076
565.340334	30.668294	72.782081
564.397248	39.193828	72.787086
563.835281	36.220856	72.792090
563.245766	26.693636	72.797095
562.330338	24.912387	72.802100
561.626191	31.807116	72.807105
560.905646	35.069532	72.812110
560.756427	31.497802	72.817114
559.478122	43.345802	72.822119
558.876829	29.403348	72.827124
558.454035	44.071911	72.832129
557.818739	42.026842	72.837134
557.589554	32.691389	72.842138
556.162893	32.227920	72.847143
555.576026	30.503151	72.852148
555.310188	30.271106	72.857153
554.464968	39.214722	72.862158
553.362432	38.067260	72.867162
552.607493	35.307958	72.872167
552.276548	42.097516	72.877172
552.107963	42.498118	72.882177
551.448198	44.758939	72.887182
550.544903	35.239119	72.892186
549.580156	42.064976	72.897191
548.993714	41.596990	72.902196
548.730048	39.331878	72.907201
548.063543	36.970082	72.912206
547.275834	32.517600	72.917210
546.528596	42.905891	72.922215
546.160446	32.414574	72.927220
545.207223	36.683896	72.932225
544.297854	34.573677	72.937230
544.130320	32.777386	72.942234
543.372137	33.152053	72.947239
542.289108	36.634641	72.952244
541.501899	36.428874	72.957249
540.946477	38.539034	72.962254
540.845780	33.297445	72.967258
540.091048	35.901406	72.972263
539.131392	37.599708	72.977268
538.466814	27.436316	72.982273
537.738484	35.249548	72.987278
537.562220	36.786796	72.992282
536.565018	31.635971	72.997287
535.803407	39.744671	73.002292
535.497021	29.814385	73.007297
534.883236	43.627111	73.012302
533.936407	24.707584	73.017306
532.970837	43.480734	73.022311
532.289360	39.157992	73.027316
532.178762	26.641823	73.032321
531.581899	40.218458	73.037326
530.576756	30.451519	73.042330
529.848482	42.574618	73.047335
529.173076	39.600801	73.052340
529.003427	34.228270	73.057345
527.999818	38.879366	73.062350
527.408743	31.331508	73.067354
526.872837	41.720832	73.072359
526.335769	32.825518	73.077364
525.534692	40.771771	73.082369
524.924837	44.981674	73.087374
524.080652	35.305792	73.092378
522.872295	40.110933	73.097383
522.417919	34.703332	73.102388
521.878675	36.560179	73.107393
521.405500	44.785366	73.112398
521.282166	36.724598	73.117402
520.108728	35.701988	73.122407
519.390094	35.778622	73.127412
518.968685	33.054512	73.132417
518.097931	37.692334	73.137422
517.471956	34.190246	73.142426
516.367207	38.702915	73.147431
515.835597	30.886963	73.152436
515.662373	33.431414	73.157441
515.303807	46.922787	73.162446
514.372813	39.501618	73.167450
513.198922	43.588481	73.172455
512.757991	40.140495	73.177460
512.511279	37.052662	73.182465
511.359654	41.470297	73.187470
510.478752	36.179529	73.192474
509.940798	42.962643	73.197479
509.449519	33.495482	73.202484
509.288074	39.868528	73.207489
508.127526	49.180942	73.212494
507.586879	38.395407	73.217498
507.136459	34.497921	73.222503
506.355810	42.608084	73.227508
505.631888	32.856283	73.232513
504.900194	40.457168	73.237518
504.667101	27.277688	73.242522
503.057164	34.250491	73.247527
502.559502	32.636105	73.252532
502.017744	30.992475	73.257537
501.477141	26.984777	73.262542
501.126301	27.586306	73.267546
500.591292	26.249111	73.272551
499.410478	41.621906	73.277556
498.696648	40.773674	73.282561
498.144531	35.663927	73.287566
497.854194	33.109755	73.292570
496.806524	40.500778	73.297575
496.148129	36.134947	73.302580
495.816926	37.331022	73.307585
495.054726	41.721320	73.312590
494.485731	23.216297	73.317594
493.450645	33.240435	73.322599
492.993642	31.342027	73.327604
492.488610	35.998866	73.332609
491.766903	44.046026	73.337614
490.828139	41.833276	73.342618
490.178474	40.375573	73.347623
490.158522	36.005808	73.352628
489.438314	33.135338	73.357633
488.268303	45.281509	73.362638
487.807018	38.758517	73.367642
487.306386	28.733031	73.372647
486.055122	34.677288	73.377652
485.596094	34.029745	73.382657
484.801753	42.646725	73.387662
484.465448	35.525075	73.392666
483.973866	38.415140	73.397671
482.858321	33.702668	73.402676
482.139794	32.675414	73.407681
481.486496	40.498784	73.412686
481.556019	31.754434	73.417690
480.791509	34.194385	73.422695
479.781240	38.950641	73.427700
479.409094	34.170201	73.432705
478.694523	43.266491	73.437710
477.758658	28.751313	73.442714
477.030455	35.619931	73.447719
476.018040	32.529508	73.452724
476.025257	30.934045	73.457729
475.450659	40.222502	73.462734
474.165240	33.726731	73.467738
473.685368	43.063178	73.472743
473.142982	30.169523	73.477748
472.854211	29.037536	73.482753
471.595971	35.850247	73.487758
471.285993	34.060886	73.492762
470.601241	39.497001	73.497767
470.222883	47.262382	73.502772
469.031893	38.226831	73.507777
468.248485	37.230419	73.512782
467.854197	41.297178	73.517786
467.407819	37.662411	73.522791
466.753661	34.519647	73.527796
465.849907	36.445616	73.532801
464.900188	31.919626	73.537806
464.768208	27.756950	73.542810
464.237774	32.696963	73.547815
463.246722	30.795335	73.552820
462.567723	25.720009	73.557825
462.022210	34.956521	73.562830
461.494378	36.587632	73.567834
460.527039	42.716907	73.572839
459.658743	31.818012	73.577844
459.424383	26.865815	73.582849
458.771337	35.088120	73.587854
458.377276	29.571578	73.592858
457.348965	30.358319	73.597863
456.994755	41.806814	73.602868
456.348520	30.446759	73.607873
454.927579	40.854091	73.612878
454.529628	31.348425	73.617882
453.968876	31.549736	73.622887
453.478365	27.414221	73.627892
452.770105	22.819806	73.632897
451.780616	41.568394	73.637902
451.524421	23.937659	73.642906
450.849289	40.933032	73.647911
450.279066	31.997292	73.652916
449.221493	30.811175	73.657921
448.466271	37.393942	73.662926
448.448280	36.868528	73.667930
447.727957	37.599896	73.672935
446.293299	36.136386	73.677940
445.831916	27.505013	73.682945
445.413560	40.914442	73.687950
445.339570	33.055562	73.692954
444.087778	36.049407	73.697959
442.893356	35.653082	73.702964
442.310786	33.102900	73.707969
442.067304	33.975918	73.712974
441.619210	32.451421	73.717978
441.095043	31.123551	73.722983
440.017497	29.376064	73.727988
439.418808	23.428501	73.732993
438.919047	33.387864	73.737998
438.458851	27.325192	73.743002
437.220032	33.029365	73.748007
436.685511	39.371965	73.753012
436.565272	31.692346	73.758017
435.838740	33.883406	73.763022
435.045829	34.582187	73.768026
434.169913	42.899936	73.773031
434.009946	29.224689	73.778036
432.780442	25.823519	73.783041
431.543002	33.227450	73.788046
431.387822	22.202338	73.793050
431.111502	23.370751	73.798055
430.291408	34.988089	73.803060
429.923872	30.851908	73.808065
429.031961	42.420770	73.813070
428.682136	31.869794	73.818074
427.680655	26.364885	73.823079
426.624666	29.231344	73.828084
426.142598	27.917270	73.833089
425.629827	37.247921	73.838094
425.282191	35.146018	73.843098
424.090181	29.490115	73.848103
423.249026	32.254535	73.853108
422.916501	30.153380	73.858113
422.485893	31.920396	73.863118
421.980718	29.763170	73.868122
420.795010	31.921739	73.873127
420.248529	34.215003	73.878132
419.870387	27.634631	73.883137
419.466429	29.861031	73.888142
418.165467	27.303895	73.893146
417.762295	30.203537	73.898151
417.010258	31.603871	73.903156
416.671206	30.136123	73.908161
415.089296	37.028817	73.913166
414.607971	24.136498	73.918170
414.061125	31.968146	73.923175
413.767690	30.051577	73.928180
413.774441	29.776114	73.933185
412.532369	40.126579	73.938190
411.816601	25.584255	73.943194
411.423245	29.102082	73.948199
410.241697	34.372937	73.953204
409.844213	26.833696	73.958209
409.211273	28.451601	73.963214
408.569199	21.028608	73.968218
408.098754	20.756642	73.973223
406.902601	33.356432	73.978228
406.406091	28.053348	73.983233
405.697862	35.535394	73.988238
405.608881	28.159888	73.993242
404.711895	20.443197	73.998247
404.021004	20.841876	74.003252
403.217577	21.055059	74.008257
402.300114	32.639029	74.013262
401.552506	31.166997	74.018266
401.214599	26.787979	74.023271
400.679153	32.269701	74.028276
400.070163	23.021613	74.033281
398.654860	41.229350	74.038286
398.175546	25.379892	74.043290
398.073015	29.884296	74.048295
397.379582	28.618101	74.053300
397.009680	29.440303	74.058305
395.867262	32.508206	74.063310
395.410400	29.037556	74.068314
394.844137	28.679933	74.073319
393.669978	31.631468	74.078324
393.182746	24.093918	74.083329
392.348439	34.087671	74.088334
392.061679	23.364233	74.093338
391.663967	34.805463	74.098343
390.309916	34.548142	74.103348
389.902162	40.186142	74.108353
389.463732	33.553879	74.113358
389.083204	22.679803	74.118362
387.718477	36.782510	74.123367
386.977348	38.602167	74.128372
386.588012	27.480329	74.133377
385.882858	39.114057	74.138382
385.761872	27.071085	74.143386
384.789830	28.766686	74.148391
383.822287	24.894863	74.153396
383.484786	27.386647	74.158401
382.567155	35.094457	74.163406
381.802917	32.395043	74.168410
381.070234	24.557560	74.173415
380.361737	38.208766	74.178420
380.440413	32.221088	74.183425
379.780427	41.013803	74.188430
378.641301	33.127542	74.193434
378.173386	34.124640	74.198439
377.720890	39.588420	74.203444
376.771186	31.642014	74.208449
375.873652	33.082892	74.213454
375.496022	37.046080	74.218458
375.155232	42.697067	74.223463
373.829160	41.724082	74.228468
373.145580	32.519423	74.233473
372.499381	43.971872	74.238478
372.106568	30.761101	74.243482
371.744382	23.086935	74.248487
370.914010	33.497962	74.253492
370.290272	33.195237	74.258497
369.633853	39.748085	74.263502
369.038431	27.466902	74.268506
368.052602	24.881654	74.273511
367.323256	36.834633	74.278516
366.926264	24.414598	74.283521
366.376356	29.133799	74.288526
365.235964	30.758464	74.293530
364.685945	30.092328	74.298535
363.913718	38.412492	74.303540
364.176205	28.431018	74.308545
362.762973	31.696635	74.313550
361.745865	24.636200	74.318554
361.271140	24.910556	74.323559
360.890656	36.967215	74.328564
360.844641	24.511751	74.333569
359.585871	31.212628	74.338574
358.633117	24.988772	74.343578
358.332237	23.404562	74.348583
358.004547	25.965749	74.353588
357.209537	29.293699	74.358593
356.020210	35.933050	74.363598
355.587080	23.291695	74.368602
355.403972	33.698926	74.373607
354.492043	23.160282	74.378612
353.504097	22.705865	74.383617
352.327184	30.986440	74.388622
352.528041	30.270031	74.393626
351.745957	29.517877	74.398631
350.694256	35.430391	74.403636
350.165012	27.487957	74.408641
349.650327	31.491912	74.413646
349.322367	25.218954	74.418650
348.393242	21.014592	74.423655
347.374967	30.723854	74.428660
347.023251	27.687471	74.433665
346.746818	28.668252	74.438670
345.841680	30.184470	74.443674
345.123646	25.175329	74.448679
344.555841	41.689978	74.453684
343.682466	27.866667	74.458689
342.742585	30.744618	74.463694
342.341285	33.617163	74.468698
341.721886	38.065168	74.473703
341.237377	40.905243	74.478708
340.855666	30.794617	74.483713
339.702494	39.123457	74.488718
339.154360	32.048215	74.493722
338.734122	35.813191	74.498727
337.366785	37.937666	74.503732
336.933892	28.120631	74.508737
336.285833	38.941013	74.513742
335.768282	35.002224	74.518746
335.794235	36.534063	74.523751
334.344322	42.659862	74.528756
333.892468	33.769951	74.533761
333.423374	39.876632	74.538766
332.701616	33.811515	74.543770
331.688130	35.822828	74.548775
330.841188	43.891557	74.553780
330.592490	32.569120	74.558785
329.875242	35.145086	74.563790
329.183622	28.568962	74.568794
328.505641	29.146956	74.573799
327.649049	37.031137	74.578804
327.905974	30.429998	74.583809
326.397792	38.432218	74.588814
325.542321	39.073195	74.593818
324.982803	36.353787	74.598823
324.478694	47.346779	74.603828
324.158750	29.641080	74.608833
323.117015	35.610364	74.613838
322.570354	31.349785	74.618842
322.213410	27.680299	74.623847
321.218932	36.242476	74.628852
320.305547	31.349632	74.633857
319.596089	38.275222	74.638862
319.358198	26.681408	74.643866
319.031114	27.846884	74.648871
318.164981	28.644105	74.653876
317.216766	17.220279	74.658881
316.570516	29.765572	74.663886
316.000204	21.824966	74.668890
315.663522	22.711271	74.673895
314.340428	22.431712	74.678900
313.660309	22.653656	74.683905
313.080019	20.577815	74.688910
313.070688	27.973719	74.693914
312.299881	24.693474	74.698919
311.047334	28.824496	74.703924
310.917877	24.778130	74.708929
310.307299	30.910514	74.713934
309.210325	30.500300	74.718938
308.400911	31.979197	74.723943
307.498491	32.853169	74.728948
307.414932	19.837569	74.733953
307.005952	32.649405	74.738958
306.497513	26.818386	74.743962
305.608472	25.980791	74.748967
304.948345	31.823025	74.753972
304.498582	23.005337	74.758977
303.109727	29.826321	74.763982
302.290693	24.305008	74.768986
301.996782	20.385781	74.773991
301.637548	29.539002	74.778996
301.338677	20.776115	74.784001
300.365849	28.901177	74.789006
299.593929	32.979256	74.794010
298.858561	16.290706	74.799015
297.816875	30.512268	74.804020
297.338445	15.725594	74.809025
296.700263	27.312382	74.814030
296.063858	30.031591	74.819034
296.057742	20.197014	74.824039
294.806271	32.192219	74.829044
294.514695	24.760708	74.834049
293.739930	26.401245	74.839054
292.432848	26.902900	74.844058
291.573886	28.832828	74.849063
291.158553	29.094577	74.854068
290.819757	26.478773	74.859073
290.390650	29.075056	74.864078
290.082289	19.898942	74.869082
289.124836	27.095875	74.874087
288.077277	29.935814	74.879092
288.102122	19.538056	74.884097
286.897191	24.159821	74.889102
286.263826	24.814295	74.894106
285.780912	17.501597	74.899111
284.829402	24.391651	74.904116
284.138884	19.584731	74.909121
282.994907	20.885147	74.914126
282.772715	22.063871	74.919130
282.384644	12.574035	74.924135
281.658456	21.047720	74.929140
281.262886	13.656448	74.934145
280.081636	21.417337	74.939150
279.783848	19.119856	74.944154
279.229277	23.402993	74.949159
278.357949	24.423408	74.954164
277.699214	14.762247	74.959169
277.036918	17.299503	74.964174
276.525459	18.685185	74.969178
275.589105	13.214126	74.974183
274.545208	18.078311	74.979188
274.367902	19.852282	74.984193
273.616311	24.863845	74.989198
273.538066	23.603709	74.994202
272.666617	10.032459	74.999207
271.310786	21.681596	75.004212
271.042848	10.641380	75.009217
270.468188	17.611717	75.014222
269.840043	19.741405	75.019226
269.174244	21.463930	75.024231
268.169089	20.220653	75.029236
268.062053	16.866162	75.034241
266.884157	29.605015	75.039246
266.174135	21.741888	75.044250
265.518641	21.471060	75.049255
264.867435	25.831106	75.054260
264.674790	25.533809	75.059265
264.081960	23.622407	75.064270
263.000076	26.245474	75.069274
262.537536	20.937015	75.074279
261.620511	25.247968	75.079284
261.489971	21.681179	75.084289
260.594388	23.170672	75.089294
259.849873	34.875346	75.094298
259.361116	26.057576	75.099303
258.709045	27.446752	75.104308
257.786014	20.510148	75.109313
257.065431	22.542609	75.114318
256.603432	22.004395	75.119322
256.551179	30.802754	75.124327
255.055635	31.973142	75.129332
254.471003	26.971152	75.134337
254.482334	28.393355	75.139342
252.951830	22.023522	75.144346
252.500214	19.365785	75.149351
251.606394	25.688408	75.154356
251.392969	29.105033	75.159361
250.717147	32.560673	75.164366
249.576458	34.866688	75.169370
249.181461	27.986263	75.174375
248.512283	21.390823	75.179380
248.375688	18.369055	75.184385
247.423439	31.715349	75.189390
246.320013	25.789955	75.194394
246.189349	22.432924	75.199399
245.622603	27.454453	75.204404
244.733205	23.439346	75.209409
243.852260	35.041190	75.214414
243.255402	28.869464	75.219418
243.091054	24.663085	75.224423
241.739484	35.242381	75.229428
241.069700	17.267635	75.234433
240.452417	24.765174	75.239438
240.116759	28.089320	75.244442
239.954626	24.238982	75.249447
238.371494	27.438708	75.254452
237.984994	22.558107	75.259457
237.461671	23.611371	75.264462
236.941760	18.263178	75.269466
236.036400	17.516521	75.274471
235.417168	24.295275	75.279476
235.080023	15.066993	75.284481
234.266790	26.708502	75.289486
233.039521	24.511888	75.294490
232.321240	23.256011	75.299495
232.063985	27.651035	75.304500
231.873100	15.493086	75.309505
231.079574	29.422790	75.314510
229.805703	23.757968	75.319514
229.290945	29.176493	75.324519
228.808018	28.371959	75.329524
228.500222	31.526083	75.334529
227.559048	32.008865	75.339534
226.808375	30.461682	75.344538
226.529702	12.970232	75.349543
225.350796	21.604408	75.354548
224.739195	23.072298	75.359553
224.012157	30.208867	75.364558
223.701009	27.342660	75.369562
223.052715	27.591095	75.374567
221.886616	32.925798	75.379572
221.168833	24.828955	75.384577
220.994699	25.608935	75.389582
220.561602	27.171372	75.394586
219.747985	35.819867	75.399591
218.559209	37.263075	75.404596
218.061400	20.771656	75.409601
217.362867	28.007761	75.414606
217.230799	31.761506	75.419610
216.190533	33.037535	75.424615
215.206554	35.509396	75.429620
214.935349	33.914166	75.434625
214.555114	27.055051	75.439630
213.493456	34.834755	75.444634
212.942259	32.561910	75.449639
212.139568	33.371132	75.454644
211.991959	31.033947	75.459649
211.036855	37.973490	75.464654
210.138759	38.835769	75.469658
209.512917	28.633210	75.474663
209.404736	35.732628	75.479668
208.129673	30.947955	75.484673
207.154287	30.368591	75.489678
206.862276	29.443737	75.494682
206.646900	24.805523	75.499687
205.994038	39.510761	75.504692
205.099528	33.755508	75.509697
204.188524	38.177489	75.514702
203.518072	35.086287	75.519706
203.215879	32.310119	75.524711
202.059132	36.083719	75.529716
201.468185	36.058086	75.534721
200.921655	37.905120	75.539726
200.445022	40.067443	75.544730
200.356080	34.082838	75.549735
199.256823	48.360930	75.554740
198.556314	38.974527	75.559745
198.090313	38.627775	75.564750
197.004908	45.529751	75.569754
196.074657	32.264364	75.574759
195.384880	43.695399	75.579764
195.083266	37.598041	75.584769
194.675381	33.197100	75.589774
193.928850	36.766530	75.594778
193.235511	35.085637	75.599783
192.523739	39.108425	75.604788
192.151255	28.012341	75.609793
191.114173	37.106481	75.614798
190.045831	41.704940	75.619802
189.931463	28.560224	75.624807
189.171403	31.672913	75.629812
188.761824	28.631591	75.634817
187.776969	35.202142	75.639822
187.041396	41.985268	75.644826
186.871361	25.506255	75.649831
185.609201	38.542431	75.654836
184.934795	34.172944	75.659841
184.399163	38.132958	75.664846
183.782162	34.476571	75.669850
183.667710	27.642899	75.674855
182.507438	43.185984	75.679860
181.686876	34.296553	75.684865
181.132777	32.913589	75.689870
180.667136	38.286447	75.694874
180.026350	33.646671	75.699879
179.110518	30.820106	75.704884
178.510806	39.287851	75.709889
177.908675	44.013838	75.714894
177.692531	43.080046	75.719898
177.138558	30.415429	75.724903
175.942778	39.334603	75.729908
175.389747	38.837726	75.734913
174.907554	29.802888	75.739918
173.556461	30.806790	75.744922
173.130896	33.534991	75.749927
172.698027	37.454968	75.754932
172.289416	34.257374	75.759937
170.995947	34.428913	75.764942
170.129607	43.145754	75.769946
170.133840	36.788325	75.774951
169.183356	49.522509	75.779956
168.777193	37.692195	75.784961
168.634129	37.185149	75.789966
167.651271	34.777709	75.794970
167.127344	32.218251	75.799975
165.714864	36.210837	75.804980
165.327628	32.763830	75.809985
165.041684	38.835021	75.814990
164.261273	39.654899	75.819994
163.348497	36.064599	75.824999
162.410393	43.695315	75.830004
161.776071	31.863538	75.835009
161.433168	34.111779	75.840014
160.638664	37.794524	75.845018
160.595263	34.464586	75.850023
159.270203	48.100595	75.855028
158.928240	32.882183	75.860033
158.643003	36.668236	75.865038
157.274396	39.761268	75.870042
156.676249	34.890771	75.875047
155.806474	29.194676	75.880052
155.639510	37.757430	75.885057
154.890182	37.247701	75.890062
153.864180	36.157606	75.895066
153.612144	32.868819	75.900071
152.656176	39.270772	75.905076
152.536811	36.217876	75.910081
151.813273	38.637196	75.915086
150.833723	38.809156	75.920090
150.330325	27.469027	75.925095
149.695963	34.303829	75.930100
148.486800	33.000089	75.935105
148.111450	31.372587	75.940110
147.195139	32.069057	75.945114
146.896594	31.364452	75.950119
146.480265	41.214349	75.955124
145.609727	31.834581	75.960129
144.986159	24.818738	75.965134
144.416630	30.991915	75.970138
143.743617	30.998305	75.975143
142.566117	33.652438	75.980148
142.078292	30.861723	75.985153
141.607138	28.740139	75.990158
141.012610	40.714239	75.995162
140.614921	26.053510	76.000167
139.612765	35.910081	76.005172
139.072372	27.600478	76.010177
138.236972	31.720261	76.015182
137.504855	33.674170	76.020186
136.904427	33.626410	76.025191
136.251182	37.070594	76.030196
135.875311	27.641921	76.035201
135.374324	25.078814	76.040206
133.910787	27.926793	76.045210
133.543837	18.572399	76.050215
132.831371	31.527246	76.055220
132.633000	34.635546	76.060225
131.807213	24.250434	76.065230
130.635429	33.214681	76.070234
130.623006	31.108263	76.075239
129.818411	34.306919	76.080244
129.437624	38.527683	76.085249
128.218114	34.659876	76.090254
127.590143	36.904691	76.095258
127.377166	28.826738	76.100263
126.293112	33.304721	76.105268
125.576555	25.359108	76.110273
125.119604	27.728040	76.115278
124.446932	34.770808	76.120282
124.508928	27.301875	76.125287
123.163429	28.000557	76.130292
122.767416	36.803261	76.135297
122.054491	27.086136	76.140302
120.731289	34.771958	76.145306
120.368018	22.367123	76.150311
119.554506	34.231058	76.155316
119.620068	28.762727	76.160321
118.378250	31.673133	76.165326
117.226458	32.741480	76.170330
116.981096	26.851217	76.175335
116.703915	34.609943	76.180340
116.274958	27.936817	76.185345
115.101190	26.534409	76.190350
114.195578	29.873757	76.195354
114.215282	34.636215	76.200359
113.199945	42.542614	76.205364
112.896007	32.842273	76.210369
111.854920	32.875826	76.215374
111.182211	36.370428	76.220378
110.686073	30.302532	76.225383
109.584818	36.360232	76.230388
109.038477	31.076209	76.235393
108.634544	26.021794	76.240398
107.986547	30.359286	76.245402
107.477465	19.236128	76.250407
106.524021	39.585959	76.255412
105.896304	32.960297	76.260417
105.404317	31.740914	76.265422
104.755484	34.902123	76.270426
103.970387	23.602202	76.275431
102.957182	29.628515	76.280436
102.661646	28.215378	76.285441
102.162673	28.958855	76.290446
101.392049	31.544970	76.295450
100.483477	32.104604	76.300455
99.877362	32.284843	76.305460
99.640957	36.321736	76.310465
98.946816	35.355365	76.315470
97.722492	31.795851	76.320474
97.616853	26.533020	76.325479
96.747236	31.050936	76.330484
96.094911	29.691542	76.335489
95.123189	28.490315	76.340494
94.494230	39.870662	76.345498
94.164740	31.926412	76.350503
93.480476	33.316033	76.355508
92.705590	32.562815	76.360513
91.854739	40.780461	76.365518
91.271656	40.677907	76.370522
91.229637	25.418000	76.375527
90.256538	34.993982	76.380532
88.912644	36.245942	76.385537
88.372147	33.342213	76.390542
87.844252	29.859304	76.395546
87.831865	25.236045	76.400551
86.936873	36.209380	76.405556
86.170138	40.439657	76.410561
85.847512	36.936629	76.415566
85.020478	35.048428	76.420570
84.029204	26.571048	76.425575
82.949342	33.863264	76.430580
82.365585	36.074229	76.435585
82.229992	35.493457	76.440590
81.642927	35.317423	76.445594
81.375403	29.787093	76.450599
80.243506	36.975645	76.455604
79.845236	30.876379	76.460609
79.035452	36.225283	76.465614
77.596660	38.291906	76.470618
77.476794	29.931028	76.475623
76.858775	42.134388	76.480628
76.264469	39.392208	76.485633
76.064824	32.215738	76.490638
74.980297	35.566286	76.495642
74.594060	29.769458	76.500647
73.886973	44.912298	76.505652
72.570572	46.710245	76.510657
72.071150	39.665159	76.515662
71.330538	30.354593	76.520666
71.425640	34.387504	76.525671
69.995239	46.073869	76.530676
69.376835	46.573047	76.535681
69.077848	41.863024	76.540686
68.660207	44.187852	76.545690
67.913988	40.933731	76.550695
66.919519	41.191682	76.555700
66.145990	43.549613	76.560705
65.982049	31.653896	76.565710
64.875813	40.875804	76.570714
64.289124	34.074877	76.575719
63.087237	35.245856	76.580724
62.811966	37.809755	76.585729
62.663572	34.444526	76.590734
61.793908	43.075192	76.595738
60.988692	26.861514	76.600743
60.421607	37.268471	76.605748
59.779560	31.707986	76.610753
59.089794	24.425183	76.615758
58.179185	26.036993	76.620762
57.892441	28.724146	76.625767
57.340538	26.019366	76.630772
56.475962	24.525098	76.635777
55.633952	24.627852	76.640782
54.826737	33.707452	76.645786
54.663109	27.528194	76.650791
53.859208	26.659767	76.655796
52.881427	25.230864	76.660801
52.658090	23.162818	76.665806
51.618970	27.089609	76.670810
51.417670	37.283687	76.675815
49.972127	36.454515	76.680820
49.578028	31.575163	76.685825
49.259418	24.587987	76.690830
48.733325	33.411440	76.695834
48.077675	21.404920	76.700839
46.804341	29.887073	76.705844
46.169838	40.136050	76.710849
46.186914	27.889769	76.715854
45.181185	33.115390	76.720858
44.249134	38.982126	76.725863
43.410884	34.736588	76.730868
42.729526	29.646007	76.735873
43.128466	28.506896	76.740878
42.243695	29.376572	76.745882
41.514781	26.031393	76.750887
40.895636	34.021281	76.755892
39.892594	32.766724	76.760897
39.053815	29.364950	76.765902
38.217640	38.062819	76.770906
37.787513	26.143334	76.775911
37.467823	33.170822	76.780916
36.813910	34.654967	76.785921
35.644171	30.664154	76.790926
34.757164	41.163143	76.795930
34.629665	34.560226	76.800935
34.003318	37.471860	76.805940
33.511819	44.547256	76.810945
32.704778	38.759201	76.815950
31.918351	33.819423	76.820954
31.674189	31.284763	76.825959
30.779737	37.066657	76.830964
29.726586	30.436336	76.835969
29.634476	31.897110	76.840974
28.840470	36.000863	76.845978
27.944725	37.604006	76.850983
26.935993	31.548501	76.855988
26.321819	38.274452	76.860993
26.262972	30.045776	76.865998
25.596619	33.190874	76.871002
24.802883	34.452893	76.876007
24.076166	29.158240	76.881012
23.341150	33.974835	76.886017
23.246389	34.526123	76.891022
21.763774	38.520512	76.896026
21.140094	31.313912	76.901031
20.681274	32.117233	76.906036
20.446420	31.545989	76.911041
19.775045	34.942628	76.916046
18.491868	42.707274	76.921050
18.148757	34.719479	76.926055
17.601087	29.549236	76.931060
16.409954	38.492962	76.936065
16.277472	32.067464	76.941070
15.561447	37.776749	76.946074
14.872961	32.600581	76.951079
14.037574	42.798026	76.956084
13.212426	36.255924	76.961089
12.927282	29.263416	76.966094
12.290142	41.282174	76.971098
11.866010	35.207548	76.976103
10.772620	35.503378	76.981108
9.876599	30.306697	76.986113
9.909851	34.248543	76.991118
9.198391	36.792132	76.996122
8.113490	29.192322	77.001127
7.302504	32.081371	77.006132
6.737232	35.147273	77.011137
6.642386	28.444537	77.016142
5.138708	33.796906	77.021147
4.372858	32.457222	77.026151
4.051714	34.408694	77.031156
3.551841	28.436041	77.036161