Thu Aug 25 16:18:02 2022

Number of Points = 9922

Depth (nm)	Load (N)	Time (s)
3.468743	100.153044	0.000000
2.968240	105.935793	0.005005
3.345301	96.347430	0.010010
3.154203	96.203392	0.015014
2.965456	95.005447	0.020019
3.199493	96.449455	0.025024
3.013884	82.969224	0.030029
3.160320	62.043231	0.035034
2.873844	71.386485	0.040038
2.490936	52.641027	0.045043
2.410233	37.432791	0.050048
1.867845	34.749504	0.055053
1.455019	10.200097	0.060058
1.149909	1.901918	0.065062
0.704241	-6.298303	0.070067
0.628128	-0.866822	0.075072
0.004407	-2.619868	0.080077
-0.513076	-11.125211	0.085082
-0.736743	-11.979155	0.090086
-1.341827	-15.601740	0.095091
-1.220056	-17.022337	0.100096
-1.477689	2.649209	0.105101
-1.679004	-9.227627	0.110106
-1.681227	-14.713214	0.115110
-2.435853	-2.620105	0.120115
-2.522391	-17.950765	0.125120
-2.928935	-1.201353	0.130125
-3.110353	-3.317931	0.135130
-3.013926	-8.537402	0.140134
-3.414800	-8.060110	0.145139
-3.656600	-17.260380	0.150144
-4.417692	-5.302302	0.155149
-4.495517	-12.747068	0.160154
-5.013322	-14.576819	0.165158
-5.315630	-6.794025	0.170163
-5.142686	-1.379421	0.175168
-4.944734	-2.005196	0.180173
-4.921187	-7.978878	0.185178
-4.742757	-11.388869	0.190182
-5.567235	-4.362654	0.195187
-5.978719	-13.542667	0.200192
-6.364362	-7.477393	0.205197
-6.791782	-6.018338	0.210202
-6.703903	-2.725946	0.215206
-7.073656	-10.634339	0.220211
-7.008079	-9.929575	0.225216
-8.063195	-10.520364	0.230221
-8.284190	-4.044288	0.235226
-8.698677	3.088534	0.240230
-9.127727	-0.764116	0.245235
-8.786742	-6.888777	0.250240
-8.663499	-2.681271	0.255245
-8.594618	-9.231534	0.260250
-9.476203	-14.085790	0.265254
-9.949903	-11.217938	0.270259
-9.891651	-13.457489	0.275264
-9.918198	-9.764354	0.280269
-10.046778	-15.008679	0.285274
-10.391826	-7.532401	0.290278
-11.094266	-1.714881	0.295283
-11.111638	-19.160279	0.300288
-11.744494	-6.428190	0.305293
-11.788019	-15.327333	0.310298
-12.454267	-12.385018	0.315302
-13.376612	0.395598	0.320307
-12.515762	-11.147786	0.325312
-12.244798	3.923084	0.330317
-13.049831	-13.933580	0.335322
-13.106833	-14.753526	0.340326
-13.155961	-6.868032	0.345331
-13.207565	-15.050898	0.350336
-14.584354	-8.649991	0.355341
-14.531972	-6.228401	0.360346
-14.512965	-2.909399	0.365350
-14.687575	3.689127	0.370355
-14.657670	-12.213441	0.375360
-15.508038	2.276985	0.380365
-16.054525	-14.845065	0.385370
-15.547136	-3.313530	0.390374
-16.240465	-1.736880	0.395379
-16.306629	-7.826220	0.400384
-16.292064	-3.130285	0.405389
-16.285925	-11.613267	0.410394
-16.913659	-9.091439	0.415398
-17.540504	-2.766907	0.420403
-17.583851	-8.157466	0.425408
-17.992496	1.274495	0.430413
-18.435205	-3.746606	0.435418
-17.981186	-7.320002	0.440422
-18.097562	3.578444	0.445427
-18.702558	-5.903445	0.450432
-18.995926	-8.236600	0.455437
-19.168083	-2.676175	0.460442
-18.910309	-10.793623	0.465446
-19.697361	-4.282637	0.470451
-19.780467	-11.448164	0.475456
-20.579681	-8.703314	0.480461
-20.636067	-3.458423	0.485466
-20.579441	-6.526626	0.490470
-21.594872	-12.767784	0.495475
-21.465546	-7.444425	0.500480
-22.074194	-0.164123	0.505485
-22.249122	-4.069244	0.510490
-22.164470	-7.208277	0.515494
-22.373729	-11.089034	0.520499
-21.981661	-9.606522	0.525504
-22.056851	-6.003841	0.530509
-22.768849	-17.449474	0.535514
-23.316835	-12.013663	0.540518
-23.876382	-3.399621	0.545523
-23.538592	-16.272083	0.550528
-23.827646	-5.340259	0.555533
-24.302612	-11.023857	0.560538
-24.918962	-4.406740	0.565542
-24.924757	-14.760797	0.570547
-25.147186	-12.457500	0.575552
-25.042268	2.854521	0.580557
-25.491558	5.237659	0.585562
-25.266682	-1.447780	0.590566
-26.171451	0.323353	0.595571
-26.433438	-11.771762	0.600576
-26.618152	2.187256	0.605581
-26.726123	-3.715199	0.610586
-26.791629	-3.391694	0.615590
-27.478636	-1.509149	0.620595
-27.803130	-5.909691	0.625600
-28.325816	0.003052	0.630605
-28.326252	-3.695291	0.635610
-27.900911	-3.366438	0.640614
-27.720287	-0.268913	0.645619
-27.993975	-4.614140	0.650624
-29.069098	0.078528	0.655629
-29.482689	-8.433600	0.660634
-29.322002	-8.148700	0.665638
-29.854358	5.529433	0.670643
-30.260857	1.068972	0.675648
-30.536154	-8.844225	0.680653
-30.901633	-6.977259	0.685658
-30.446394	-5.112338	0.690662
-30.984378	5.241562	0.695667
-31.126263	-10.039299	0.700672
-31.600159	-5.602189	0.705677
-32.413898	-4.598295	0.710682
-32.278292	9.598441	0.715686
-32.664154	-1.809716	0.720691
-32.648387	-5.311280	0.725696
-32.652204	-1.602723	0.730701
-32.911719	1.108185	0.735706
-32.635195	-4.009791	0.740710
-33.255648	4.645435	0.745715
-33.421422	-13.472741	0.750720
-34.001352	-1.783492	0.755725
-34.392313	-0.627542	0.760730
-34.605989	0.921410	0.765734
-35.289190	2.537603	0.770739
-35.208385	-8.573510	0.775744
-35.086425	5.884789	0.780749
-35.825463	-1.785406	0.785754
-35.609926	-7.403191	0.790758
-35.997109	-5.216447	0.795763
-36.565482	-1.612420	0.800768
-36.880268	8.488210	0.805773
-36.866892	-6.532243	0.810778
-36.640992	0.579329	0.815782
-36.794913	-4.347813	0.820787
-37.490195	5.575152	0.825792
-38.209413	8.683959	0.830797
-38.236985	6.068711	0.835802
-38.082212	-0.061576	0.840806
-38.808788	7.044217	0.845811
-38.369418	-0.570176	0.850816
-38.954187	11.819031	0.855821
-39.630325	-0.230180	0.860826
-39.870075	0.073171	0.865830
-40.177915	-0.489171	0.870835
-39.968667	-4.691769	0.875840
-40.462590	1.238613	0.880845
-40.323127	-3.658570	0.885850
-40.520332	-6.943264	0.890854
-41.003660	-6.544800	0.895859
-41.291646	-4.560261	0.900864
-41.703543	-2.037449	0.905869
-41.396760	-1.427427	0.910874
-41.902343	-3.053447	0.915878
-42.756937	6.400934	0.920883
-42.650422	-12.171195	0.925888
-42.564229	2.609080	0.930893
-42.850230	9.206078	0.935898
-42.645738	-6.293575	0.940902
-43.885473	-7.428073	0.945907
-44.342770	-11.462953	0.950912
-44.530890	-3.527208	0.955917
-44.750038	0.192943	0.960922
-44.171559	-5.143189	0.965926
-44.928114	2.558923	0.970931
-44.655981	-3.675173	0.975936
-45.217223	-1.628834	0.980941
-45.632863	-1.683902	0.985946
-45.747591	-0.055542	0.990950
-46.020961	3.378875	0.995955
-46.317664	-3.996794	1.000960
-46.871305	-5.346364	1.005965
-47.556811	-0.749544	1.010970
-47.307358	-3.452491	1.015974
-47.542607	1.595799	1.020979
-47.253996	-5.004711	1.025984
-47.523584	-6.341841	1.030989
-47.603785	0.868314	1.035994
-48.221535	-4.150667	1.040998
-48.710022	-0.258599	1.046003
-48.698684	-8.416527	1.051008
-48.874584	-5.611154	1.056013
-49.325298	0.802841	1.061018
-49.633311	-6.675459	1.066022
-50.550048	-3.260456	1.071027
-50.280095	-7.080259	1.076032
-50.515142	-1.358120	1.081037
-50.582751	-2.173240	1.086042
-50.312091	-7.622491	1.091046
-50.904031	-3.122590	1.096051
-51.316346	-11.090747	1.101056
-51.796856	-6.193855	1.106061
-52.049972	-6.793246	1.111066
-52.025022	-9.578073	1.116070
-52.175199	-3.954655	1.121075
-52.417390	-14.822162	1.126080
-53.208977	-6.260349	1.131085
-53.069029	-8.715182	1.136090
-53.534048	-8.841606	1.141094
-53.674813	-0.166632	1.146099
-53.341143	2.391219	1.151104
-53.525863	-5.033634	1.156109
-54.360605	-7.731212	1.161114
-54.225897	-7.426424	1.166118
-54.842677	2.598135	1.171123
-54.776514	-8.412605	1.176128
-55.474263	-5.436878	1.181133
-56.006472	-3.274866	1.186138
-56.365919	-0.295199	1.191142
-56.323034	-0.561318	1.196147
-56.266727	-2.797401	1.201152
-56.132917	-1.344026	1.206157
-56.781658	-5.016714	1.211162
-57.324278	-1.970381	1.216166
-57.872097	-3.966270	1.221171
-57.981792	-2.310224	1.226176
-57.541534	4.084388	1.231181
-57.804308	-0.559943	1.236186
-57.969910	-2.894133	1.241190
-58.570172	8.216175	1.246195
-59.050754	-3.648535	1.251200
-59.261649	-0.530793	1.256205
-59.295502	-3.445613	1.261210
-59.221058	-4.640496	1.266214
-60.264775	-3.657512	1.271219
-60.872483	-8.735011	1.276224
-60.297961	0.609333	1.281229
-60.655163	-7.959083	1.286234
-60.638756	-5.025655	1.291238
-61.287556	-8.979907	1.296243
-61.137260	-0.616296	1.301248
-61.285291	-1.415651	1.306253
-61.928642	1.320600	1.311258
-62.354078	-5.661572	1.316262
-62.450711	3.329192	1.321267
-62.164234	6.315218	1.326272
-62.507151	-11.730905	1.331277
-63.523383	-5.851562	1.336282
-63.808139	-7.043945	1.341286
-64.301086	-2.088155	1.346291
-64.006450	-15.425254	1.351296
-64.158253	6.763877	1.356301
-64.054126	-2.550710	1.361306
-63.795469	-3.543504	1.366310
-64.591725	-2.064618	1.371315
-65.170758	-2.492717	1.376320
-65.728542	2.406795	1.381325
-65.904355	-3.937446	1.386330
-65.710274	-4.236748	1.391334
-65.862555	-0.391034	1.396339
-66.319120	-4.925903	1.401344
-66.644510	1.174225	1.406349
-66.890142	4.088603	1.411354
-66.765448	-5.833483	1.416358
-67.655268	5.670208	1.421363
-68.152074	-3.509088	1.426368
-68.308381	-1.684386	1.431373
-68.612355	2.333794	1.436378
-68.408738	-1.817301	1.441382
-68.577708	-3.401151	1.446387
-68.661982	-7.972208	1.451392
-68.532322	-8.742308	1.456397
-68.726299	-8.560024	1.461402
-69.508878	-14.236544	1.466406
-70.092445	-2.565710	1.471411
-70.220932	-6.199693	1.476416
-70.579743	-4.223039	1.481421
-71.156155	-0.848706	1.486426
-71.159659	-12.348400	1.491430
-71.620844	-0.971989	1.496435
-71.702212	-16.711575	1.501440
-71.818489	-4.234438	1.506445
-71.927480	-3.328315	1.511450
-71.646307	-7.988272	1.516454
-71.830549	-8.402300	1.521459
-72.090846	-8.737973	1.526464
-72.531947	3.859670	1.531469
-73.227876	2.681095	1.536474
-73.180922	0.914714	1.541478
-74.236790	2.121067	1.546483
-74.495695	-0.565499	1.551488
-74.459983	-3.864543	1.556493
-75.032595	-2.063195	1.561498
-74.817330	-5.507432	1.566502
-75.143294	3.699601	1.571507
-75.136675	0.259582	1.576512
-74.636392	-1.112759	1.581517
-74.929902	4.514138	1.586522
-75.038922	-11.243267	1.591526
-76.066247	0.443319	1.596531
-76.276745	-2.557717	1.601536
-77.276569	-6.403181	1.606541
-77.333841	-2.357219	1.611546
-77.404712	-4.990990	1.616550
-77.671414	6.424555	1.621555
-77.517737	-1.436137	1.626560
-77.419905	-3.748329	1.631565
-77.794868	6.757197	1.636570
-78.397858	-4.645402	1.641574
-78.903043	2.346605	1.646579
-78.970493	-0.695828	1.651584
-78.393430	1.314517	1.656589
-79.592796	-0.547640	1.661594
-79.702521	-5.668367	1.666598
-80.350448	9.344000	1.671603
-80.151725	-3.269394	1.676608
-80.058356	-6.308552	1.681613
-80.542906	4.236291	1.686618
-80.727794	-5.586665	1.691622
-81.634533	-3.432404	1.696627
-81.641142	-11.293285	1.701632
-81.681141	-7.480985	1.706637
-81.708253	-3.284725	1.711642
-81.625543	-1.516459	1.716646
-82.262295	3.167636	1.721651
-82.820995	-2.869834	1.726656
-82.984516	-6.748264	1.731661
-83.328585	3.315820	1.736666
-83.361542	-10.172430	1.741670
-83.670432	-5.280282	1.746675
-83.897357	-5.643330	1.751680
-84.201665	-7.769122	1.756685
-84.576407	-3.898041	1.761690
-84.770276	-15.908906	1.766694
-84.631773	-7.154310	1.771699
-85.232815	-2.254349	1.776704
-85.618209	-2.162294	1.781709
-85.947064	-2.575808	1.786714
-85.894706	-8.936816	1.791718
-86.200760	-2.203804	1.796723
-86.437808	3.104197	1.801728
-86.486503	0.723215	1.806733
-86.925250	-5.902527	1.811738
-87.585481	-4.185526	1.816742
-87.883080	14.160339	1.821747
-87.890061	-4.533213	1.826752
-87.864204	-2.278310	1.831757
-88.082002	2.270534	1.836762
-87.810190	-7.516414	1.841766
-88.181653	0.318346	1.846771
-88.838993	0.978198	1.851776
-88.858608	-1.666768	1.856781
-89.577459	4.947431	1.861786
-89.916063	-4.471786	1.866790
-90.201095	-1.816991	1.871795
-90.833966	-0.980639	1.876800
-90.599599	-6.427366	1.881805
-91.044593	-4.826349	1.886810
-90.703691	-14.288761	1.891814
-91.127812	1.742062	1.896819
-91.133700	-2.629305	1.901824
-91.309241	-8.612916	1.906829
-91.978628	-12.139995	1.911834
-92.041487	-9.346008	1.916838
-92.431234	-9.740489	1.921843
-92.487170	-6.640702	1.926848
-93.339641	-4.634149	1.931853
-93.591370	-8.970157	1.936858
-93.408572	-19.135457	1.941862
-94.367466	-11.180180	1.946867
-94.090319	-13.213584	1.951872
-94.036293	-3.620009	1.956877
-94.017608	-1.174157	1.961882
-93.850384	-12.782859	1.966886
-94.949860	-6.896797	1.971891
-94.975196	-11.821937	1.976896
-95.212737	-0.360347	1.981901
-95.870096	-3.259723	1.986906
-96.283434	-9.414879	1.991910
-96.882399	-4.094463	1.996915
-96.318172	-9.002542	2.006912
-96.097164	-6.110059	2.016909
-95.617384	-10.027736	2.026906
-95.282324	-10.032664	2.036902
-95.078289	-4.752159	2.046899
-94.614462	-12.180439	2.056896
-93.406983	-12.261883	2.066893
-93.013845	-9.051080	2.076890
-92.634406	-12.145242	2.086886
-92.425835	-10.562284	2.096883
-91.677627	-12.447106	2.106880
-91.390257	-9.805775	2.116877
-90.830507	-14.553277	2.126874
-90.485079	1.219040	2.136870
-89.800620	-2.182680	2.146867
-89.076297	-8.663422	2.156864
-88.813892	-3.316035	2.166861
-88.093231	-4.182841	2.176858
-87.447027	-11.566839	2.186854
-87.599826	-0.661406	2.196851
-86.606897	-3.306836	2.206848
-86.044939	-9.223609	2.216845
-86.106396	-7.959469	2.226842
-85.099467	-6.384399	2.236838
-84.573579	-6.922910	2.246835
-84.342450	-2.989801	2.256832
-83.458479	-4.747009	2.266829
-83.417796	-3.799816	2.276826
-82.936417	-0.761228	2.286822
-81.634555	-2.888027	2.296819
-81.746748	-0.849326	2.306816
-81.604325	-1.134514	2.316813
-80.511105	-4.628794	2.326810
-80.051282	-4.840172	2.336806
-79.981220	-11.335603	2.346803
-79.060702	-8.638259	2.356800
-78.905588	-8.108140	2.366797
-78.107195	-11.065210	2.376794
-77.348058	-8.719547	2.386790
-77.125887	-8.754303	2.396787
-77.038252	-13.465842	2.406784
-76.187699	-12.731081	2.416781
-75.698692	-10.526824	2.426778
-74.774245	-12.854243	2.436774
-74.366145	-13.941336	2.446771
-74.237720	-13.058576	2.456768
-74.159466	-12.101431	2.466765
-73.605735	-9.223068	2.476762
-72.701805	-10.432203	2.486758
-72.027434	-14.789017	2.496755
-71.818645	-5.010964	2.506752
-70.843661	-10.466597	2.516749
-70.246011	-5.656414	2.526746
-70.306878	-9.875849	2.536742
-70.137004	-9.005919	2.546739
-69.058846	-10.159991	2.556736
-68.791092	-7.940072	2.566733
-68.013316	-3.291161	2.576730
-67.536772	0.261372	2.586726
-67.309408	-4.339016	2.596723
-66.808478	-0.600236	2.606720
-66.361985	-3.286755	2.616717
-64.982865	-1.459556	2.626714
-65.022134	0.292120	2.636710
-64.165767	-9.852297	2.646707
-64.198238	-2.371115	2.656704
-64.263590	-5.569812	2.666701
-63.252111	-7.714464	2.676698
-62.728111	-6.291803	2.686694
-62.092930	-5.634166	2.696691
-61.508643	-9.900838	2.706688
-61.236161	-4.878145	2.716685
-60.319986	-11.997167	2.726682
-60.154355	3.603758	2.736678
-60.128289	-8.723063	2.746675
-58.906837	-6.902836	2.756672
-58.672214	-1.737994	2.766669
-58.118920	-4.336709	2.776666
-57.359409	-5.801981	2.786662
-57.151640	-5.115386	2.796659
-56.955046	-10.208298	2.806656
-56.286722	-5.583417	2.816653
-56.042302	-1.969170	2.826650
-54.876226	-2.937444	2.836646
-54.465234	-4.569854	2.846643
-54.269347	-6.095698	2.856640
-53.409353	-4.931591	2.866637
-52.957141	-0.098616	2.876634
-52.878001	-0.896577	2.886630
-51.890925	1.432380	2.896627
-51.686850	-4.868642	2.906624
-51.003161	-3.879649	2.916621
-50.373459	-3.569613	2.926618
-50.167369	-4.020000	2.936614
-50.066715	-8.546679	2.946611
-48.995397	0.123711	2.956608
-48.810730	-7.726498	2.966605
-48.200899	-5.452472	2.976602
-47.278366	-2.403811	2.986598
-47.177465	-1.624443	2.996595
-46.609386	-6.240203	3.006592
-46.044945	-4.437404	3.016589
-45.880996	2.097507	3.026586
-44.969380	1.663284	3.036582
-44.386969	4.042978	3.046579
-44.418292	0.845283	3.056576
-43.598111	1.195166	3.066573
-43.020377	-6.390349	3.076570
-42.787729	-8.188049	3.086566
-41.840287	-1.218370	3.096563
-41.480225	-6.590322	3.106560
-41.170714	-3.198517	3.116557
-40.120681	1.109965	3.126554
-39.754582	-4.088704	3.136550
-39.559487	-9.799105	3.146547
-39.610766	-6.157532	3.156544
-38.774583	-5.129076	3.166541
-38.344726	-2.548080	3.176538
-37.249459	-5.998326	3.186534
-36.975241	-2.873423	3.196531
-36.728979	-0.960579	3.206528
-35.719594	1.583465	3.216525
-35.050020	-3.659587	3.226522
-35.323137	-1.095156	3.236518
-35.041595	-7.031347	3.246515
-33.937768	-3.295165	3.256512
-33.668701	-2.960298	3.266509
-33.040973	-6.964513	3.276506
-32.688688	-5.125303	3.286502
-32.177654	0.921234	3.296499
-31.509983	-2.854822	3.306496
-30.912837	-1.731890	3.316493
-30.529951	-1.814001	3.326490
-29.622566	-5.453387	3.336486
-29.478258	-5.136985	3.346483
-29.346890	-8.790994	3.356480
-28.615215	-7.834861	3.366477
-27.995810	-8.904376	3.376474
-27.878034	-3.198534	3.386470
-26.647310	-14.361452	3.396467
-26.188678	-12.580087	3.406464
-26.474209	-8.835286	3.416461
-25.836809	-5.076705	3.426458
-25.374334	-7.968466	3.436454
-24.308805	-9.782626	3.446451
-23.782895	-6.598957	3.456448
-23.540947	-9.554367	3.466445
-23.214736	-2.781952	3.476442
-22.461612	-3.010773	3.486438
-22.061697	-2.541185	3.496435
-21.908076	-5.162806	3.506432
-20.777969	-1.433907	3.516429
-20.651394	-4.726035	3.526426
-19.946969	-0.319049	3.536422
-19.192308	-6.604971	3.546419
-19.236371	-4.519925	3.556416
-18.423281	2.277575	3.566413
-17.835269	-2.734118	3.576410
-17.872721	-8.072295	3.586406
-17.098557	-7.816569	3.596403
-16.344636	-2.935831	3.606400
-16.215627	-8.727745	3.616397
-15.276720	-2.469482	3.626394
-15.003206	-3.459457	3.636390
-14.668272	-5.510771	3.646387
-13.875622	-6.978064	3.656384
-13.366137	-9.547737	3.666381
-13.179389	-7.318290	3.676378
-12.276247	-10.899988	3.686374
-11.450150	-11.802315	3.696371
-11.333517	-6.796381	3.706368
-11.386782	-5.425818	3.716365
-10.600758	-3.923831	3.726362
-9.845227	-14.885580	3.736358
-9.869027	-10.158585	3.746355
-9.039325	-9.873547	3.756352
-8.647242	-6.139883	3.766349
-8.399325	2.627854	3.776346
-7.621842	-3.677484	3.786342
-6.655021	-5.910168	3.796339
-5.781292	-1.510701	3.806336
-6.156067	-11.997575	3.816333
-5.968387	-2.168688	3.826330
-5.445538	-0.495584	3.836326
-4.746561	2.461399	3.846323
-3.839565	12.297966	3.856320
-4.013643	13.012714	3.866317
-3.304298	36.052053	3.876314
-2.973668	38.997065	3.886310
-2.506881	53.793747	3.896307
-1.988325	67.508436	3.906304
-1.378410	79.358809	3.916301
-1.203644	90.111610	3.926298
-0.594503	112.536350	3.936294
0.000000	120.628679	3.941299
-0.493077	140.109473	3.946304
0.244157	142.088417	3.951309
0.582099	152.377927	3.956314
0.265897	156.182920	3.961318
0.641228	154.763709	3.966323
0.461875	165.887261	3.971328
0.820473	157.174965	3.976333
0.752740	158.501744	3.981338
0.861446	152.109699	3.986342
0.820441	149.319361	3.991347
0.649593	166.386344	3.996352
0.514372	160.250818	4.001357
0.536255	163.613694	4.006362
0.623472	174.243061	4.011366
1.135591	174.257762	4.016371
1.082495	186.212605	4.021376
1.355931	181.145681	4.026381
1.110335	168.370819	4.031386
0.896284	157.505118	4.036390
0.755193	153.243479	4.041395
0.582894	168.491512	4.046400
0.766187	174.670186	4.051405
1.407505	183.365084	4.056410
1.091898	185.977239	4.061414
1.130397	161.040529	4.066419
1.113442	164.425309	4.071424
0.863253	160.835668	4.076429
1.102239	175.974972	4.081434
0.994965	172.935582	4.086438
1.368278	172.551248	4.091443
0.880609	169.625245	4.096448
1.265890	168.043121	4.101453
0.807538	167.191138	4.106458
0.898032	183.492681	4.111462
1.286882	177.132664	4.116467
1.028641	182.997704	4.121472
1.007370	175.278239	4.126477
1.140011	186.871781	4.131482
1.172134	189.704703	4.136486
1.218230	186.258461	4.141491
0.782346	193.885099	4.146496
1.235649	196.338814	4.151501
1.262520	190.582846	4.156506
1.199390	194.503221	4.161510
1.012704	197.123652	4.166515
0.848830	191.017915	4.171520
0.951769	185.433530	4.176525
1.196926	195.737603	4.181530
0.974823	195.183965	4.186534
1.462554	198.714305	4.191539
1.461513	210.812870	4.196544
1.553073	208.681969	4.201549
1.270949	190.233793	4.206554
1.276957	194.026274	4.211558
1.634956	205.179553	4.216563
1.536232	206.492208	4.221568
1.413309	199.570118	4.226573
1.403404	191.858357	4.231578
1.285663	189.159131	4.236582
1.601375	184.920824	4.241587
1.337419	198.139431	4.246592
1.540858	205.858894	4.251597
1.364705	195.135931	4.256602
1.522124	208.658686	4.261606
1.978067	206.907297	4.266611
1.618743	206.640919	4.271616
1.530468	191.775428	4.276621
1.276592	187.623203	4.281626
1.542106	193.681432	4.286630
1.690964	194.724338	4.291635
1.290100	196.878446	4.296640
1.198537	207.896518	4.301645
1.829048	201.523939	4.306650
1.855175	217.421140	4.311654
1.969493	208.816698	4.316659
1.262322	221.218902	4.321664
1.808492	216.204149	4.326669
2.174261	211.603647	4.331674
1.521762	204.327927	4.336678
1.647736	185.496269	4.341683
1.497464	203.670557	4.346688
1.770030	216.219809	4.351693
2.142363	206.856757	4.356698
1.676978	200.545155	4.361702
1.697665	197.934971	4.366707
1.794688	212.549213	4.371712
2.020428	213.852159	4.376717
1.799394	199.573785	4.381722
1.754868	195.031246	4.386726
1.557584	194.821737	4.391731
1.683988	210.738022	4.396736
2.024747	215.398725	4.401741
2.071284	221.367886	4.406746
1.851007	221.665024	4.411750
2.056847	213.429059	4.416755
1.852689	212.379056	4.421760
2.044242	220.059258	4.426765
1.855867	214.042775	4.431770
1.694935	213.207465	4.436774
2.187021	214.038402	4.441779
1.895533	220.538260	4.446784
2.160362	211.021205	4.451789
2.241115	215.058248	4.456794
2.338881	213.385125	4.461798
2.012338	187.885470	4.466803
1.499807	198.425322	4.471808
1.477472	201.842590	4.476813
1.910774	213.411188	4.481818
2.227807	207.818562	4.486822
1.960725	205.620466	4.491827
1.651888	220.004072	4.496832
1.568423	216.328184	4.501837
1.643042	220.404154	4.506842
1.914979	215.334292	4.511846
2.484468	213.239240	4.516851
2.094634	219.931679	4.521856
1.805199	222.970016	4.526861
2.419543	224.480999	4.531866
1.810901	230.527509	4.536870
2.186413	226.820834	4.541875
2.118760	244.934761	4.546880
2.525675	242.776592	4.551885
2.485839	246.658527	4.556890
2.304302	222.031459	4.561894
2.295185	224.326674	4.566899
2.188010	235.891384	4.571904
2.308937	231.658276	4.576909
2.226975	229.051516	4.581914
2.545321	233.491105	4.586918
2.605533	226.910475	4.591923
2.015435	230.407217	4.596928
2.352640	238.744824	4.601933
2.600431	240.566346	4.606938
2.159243	230.049407	4.611942
2.298649	225.541317	4.616947
2.358035	236.273160	4.621952
2.587651	231.757262	4.626957
2.596921	243.183507	4.631962
2.533612	242.741031	4.636966
2.595063	229.823102	4.641971
2.355584	225.190877	4.646976
2.303961	223.471557	4.651981
2.360076	236.883654	4.656986
2.882778	239.769435	4.661990
2.462769	231.084184	4.666995
2.295374	232.875844	4.672000
2.432608	239.147181	4.677005
2.740161	242.863951	4.682010
2.610925	244.706582	4.687014
3.027697	243.217596	4.692019
2.552014	242.267082	4.697024
2.442432	220.675490	4.702029
2.581641	222.567808	4.707034
2.488616	230.931692	4.712038
2.985672	241.990438	4.717043
2.776248	238.384902	4.722048
2.767863	230.634919	4.727053
2.556239	220.275009	4.732058
2.624632	220.071329	4.737062
2.900741	221.891576	4.742067
2.628595	223.171293	4.747072
2.212378	224.922843	4.752077
2.613312	231.295231	4.757082
2.282897	247.646963	4.762086
2.693027	246.782287	4.767091
2.603072	246.432572	4.772096
2.777319	247.968220	4.777101
2.684079	246.033952	4.782106
2.569809	253.983553	4.787110
2.654262	245.902637	4.792115
2.652736	251.676855	4.797120
2.795757	242.944511	4.802125
2.890064	244.328166	4.807130
3.082447	256.143351	4.812134
2.936544	249.487439	4.817139
2.716379	245.054667	4.822144
2.752348	248.776025	4.827149
2.982598	238.701216	4.832154
2.798542	254.077716	4.837158
3.194394	259.248662	4.842163
2.899715	262.689631	4.847168
3.060809	255.779967	4.852173
3.096038	249.826515	4.857178
2.929977	247.232929	4.862182
3.152734	245.923040	4.867187
2.704394	257.003372	4.872192
3.064336	264.059249	4.877197
2.935283	275.617921	4.882202
3.169689	269.028966	4.887206
3.318254	279.455791	4.892211
3.359088	272.590275	4.897216
2.859114	256.723032	4.902221
3.134257	255.325839	4.907226
3.217209	277.706329	4.912230
3.110539	254.364651	4.917235
2.901440	263.623112	4.922240
3.145011	276.461693	4.927245
3.384856	269.077769	4.932250
3.475399	275.631686	4.937254
3.304142	248.892707	4.942259
3.182180	251.844696	4.947264
3.142879	244.789262	4.952269
3.067899	249.455001	4.957274
3.215150	260.362919	4.962278
2.979845	263.683852	4.967283
3.092751	264.124942	4.972288
3.037727	268.778068	4.977293
3.346080	269.394183	4.982298
3.437458	271.490157	4.987302
3.475635	262.644513	4.992307
3.208429	277.638586	4.997312
3.132958	272.129585	5.002317
3.532976	272.187162	5.007322
3.418602	273.695267	5.012326
3.553638	263.983381	5.017331
3.551897	273.835793	5.022336
3.403785	266.234241	5.027341
3.558162	270.829247	5.032346
3.540214	268.905326	5.037350
3.589679	269.017829	5.042355
3.253371	279.988870	5.047360
3.362003	284.043707	5.052365
3.409642	277.512486	5.057370
3.417849	281.412212	5.062374
3.514873	277.793454	5.067379
3.477045	282.592588	5.072384
3.690412	272.820967	5.077389
3.712265	277.958768	5.082394
3.737046	272.952925	5.087398
3.324465	273.004943	5.092403
3.547796	272.694727	5.097408
3.331356	280.116173	5.102413
3.712927	279.528058	5.107418
3.320554	279.064372	5.112422
3.720512	266.586932	5.117427
3.484324	280.895928	5.122432
3.489768	267.154664	5.127437
3.799659	279.068513	5.132442
3.849214	283.078821	5.137446
3.689824	271.432516	5.142451
3.482569	274.641486	5.147456
3.557032	273.883187	5.152461
3.456606	278.170099	5.157466
3.278202	294.469582	5.162470
3.689251	300.783461	5.167475
3.412917	309.793048	5.172480
3.633396	308.534133	5.177485
3.875491	308.667075	5.182490
3.755064	305.759440	5.187494
4.104328	299.424566	5.192499
4.023797	313.475076	5.197504
3.526982	308.446543	5.202509
3.868171	310.323042	5.207514
3.704600	303.391462	5.212518
3.894479	295.331971	5.217523
3.822982	305.688886	5.222528
3.385048	306.247923	5.227533
3.623044	294.627925	5.232538
3.703771	308.156445	5.237542
3.648459	312.528047	5.242547
3.808608	320.165756	5.247552
3.828824	326.006196	5.252557
4.110289	322.693895	5.257562
3.958237	330.693743	5.262566
4.128194	325.367740	5.267571
4.331097	326.870430	5.272576
3.884512	323.279890	5.277581
3.842648	322.207614	5.282586
3.971747	329.306015	5.287590
4.098586	321.617065	5.292595
3.656016	325.441894	5.297600
4.017165	329.659660	5.302605
4.191244	323.810980	5.307610
4.015395	322.342074	5.312614
4.112394	326.281681	5.317619
4.022113	330.228487	5.322624
3.993793	317.084109	5.327629
4.274252	324.794720	5.332634
3.690567	327.683022	5.337638
3.832726	326.679991	5.342643
3.811105	338.538253	5.347648
4.326396	343.810736	5.352653
4.707237	349.619990	5.357658
4.457917	355.439394	5.362662
4.519848	348.640147	5.367667
4.485736	337.211456	5.372672
4.140415	337.888864	5.377677
4.164289	325.258334	5.382682
4.262698	336.673836	5.387686
4.569229	322.705015	5.392691
4.278761	332.520439	5.397696
4.309607	328.253965	5.402701
4.893535	333.120212	5.407706
4.636742	331.790541	5.412710
4.308855	329.991107	5.417715
4.347751	325.286765	5.422720
4.507745	327.014483	5.427725
4.547300	328.928754	5.432730
4.264487	323.648382	5.437734
4.293682	337.058445	5.442739
4.183835	325.647956	5.447744
4.365461	331.735195	5.452749
4.339540	337.389874	5.457754
4.483320	345.375016	5.462758
4.458008	354.101679	5.467763
4.568954	347.952829	5.472768
4.813158	351.590961	5.477773
4.861505	338.067551	5.482778
4.749470	340.255517	5.487782
4.449883	331.627281	5.492787
4.542637	330.755381	5.497792
4.297452	334.311997	5.502797
4.510901	345.187449	5.507802
4.585440	343.204735	5.512806
4.570387	357.371573	5.517811
4.624865	353.895511	5.522816
4.706275	356.834635	5.527821
4.661403	353.196965	5.532826
4.664938	346.704268	5.537830
5.081836	353.124819	5.542835
4.531954	351.040620	5.547840
4.571616	354.457695	5.552845
4.756813	347.610660	5.557850
4.591325	357.384368	5.562854
4.424090	354.775131	5.567859
4.462267	356.227703	5.572864
4.625961	358.707835	5.577869
4.887027	352.864499	5.582874
4.442145	361.308885	5.587878
4.619426	358.496968	5.592883
4.801421	355.051547	5.597888
4.563320	364.175396	5.602893
5.211490	367.126962	5.607898
4.638558	375.961586	5.612902
4.719388	378.989392	5.617907
5.211615	386.416906	5.622912
4.759899	387.506466	5.627917
4.879523	380.305852	5.632922
4.901553	386.376986	5.637926
4.747159	387.476909	5.642931
4.986001	386.180309	5.647936
4.789508	378.589453	5.652941
5.044573	380.027027	5.657946
5.100272	371.963214	5.662950
4.971977	374.280286	5.667955
5.208455	378.141102	5.672960
5.198076	379.313374	5.677965
5.256409	372.631743	5.682970
4.883318	382.937879	5.687974
4.997045	369.726912	5.692979
4.854225	372.561963	5.697984
4.976578	383.929450	5.702989
5.470191	374.642224	5.707994
4.921782	381.195051	5.712998
4.770806	374.599999	5.718003
5.140959	382.480084	5.723008
5.128435	386.655170	5.728013
4.760903	375.762763	5.733018
4.723246	383.222679	5.738022
5.161431	375.598821	5.743027
5.199218	383.622733	5.748032
4.719007	399.656381	5.753037
5.312504	407.697640	5.758042
5.246376	407.527691	5.763046
4.934470	407.231732	5.768051
5.315651	394.557824	5.773056
5.271594	402.803382	5.778061
5.476028	402.106973	5.783066
5.235094	411.531855	5.788070
5.140906	400.337169	5.793075
5.651583	401.544864	5.798080
4.924082	409.530504	5.803085
5.339181	411.825716	5.808090
5.011275	417.356889	5.813094
4.922793	408.695539	5.818099
5.241162	405.804559	5.823104
5.362067	416.634442	5.828109
5.504715	407.579364	5.833114
5.163103	413.062062	5.838118
5.466162	429.207134	5.843123
5.582594	433.969483	5.848128
5.523363	440.385572	5.853133
6.110684	439.116627	5.858138
5.821873	426.092080	5.863142
5.563156	413.591189	5.868147
5.297953	412.345088	5.873152
5.272551	418.891914	5.878157
5.343619	414.413467	5.883162
5.217674	419.539665	5.888166
5.734572	432.117227	5.893171
5.928793	432.539253	5.898176
5.484912	430.182165	5.903181
5.871844	423.385752	5.908186
5.989524	420.931186	5.913190
5.408717	410.543585	5.918195
5.731512	425.189067	5.923200
5.223212	418.023546	5.928205
5.392471	428.039081	5.933210
5.541575	435.460264	5.938214
5.700858	436.466748	5.943219
5.934144	434.484462	5.948224
5.436606	439.045610	5.953229
5.888055	437.076599	5.958234
6.035614	441.796107	5.963238
5.726884	445.656939	5.968243
5.762487	439.171839	5.973248
5.601350	447.103559	5.978253
6.015633	443.526810	5.983258
5.954203	449.620534	5.988262
5.682025	439.371227	5.993267
5.750097	423.294606	5.998272
5.855924	415.371621	6.003277
5.863941	410.213338	6.008282
5.780256	421.774487	6.013286
5.415108	409.758523	6.018291
5.436857	423.900664	6.023296
5.582396	439.311105	6.028301
5.848669	436.355514	6.033306
5.980890	438.929176	6.038310
5.416851	434.692609	6.043315
5.718860	435.989950	6.048320
5.797553	443.722735	6.053325
5.931189	447.112448	6.058330
5.638104	433.196361	6.063334
5.874292	420.263571	6.068339
6.040246	419.513078	6.073344
5.627821	424.393090	6.078349
5.709013	408.032846	6.083354
5.689814	410.111359	6.088358
5.423701	415.405054	6.093363
5.357387	425.261339	6.098368
5.093353	436.910869	6.103373
5.829504	444.746291	6.108378
5.813273	448.611915	6.113382
6.076493	438.892506	6.118387
5.805529	444.019285	6.123392
5.537335	447.038512	6.128397
5.988283	443.927431	6.133402
5.614700	442.986219	6.138406
5.503219	445.784733	6.143411
5.545105	445.395374	6.148416
5.459233	449.961628	6.153421
5.491172	447.586933	6.158426
5.514288	449.127295	6.163430
5.646443	449.258482	6.168435
5.672703	434.858912	6.173440
5.446684	449.419555	6.178445
5.768712	438.140649	6.183450
5.521245	437.891542	6.188454
5.604783	434.429894	6.193459
5.552751	443.610053	6.198464
5.528335	449.473345	6.203469
5.832112	444.445887	6.208474
5.879986	448.602033	6.213478
5.987203	452.701423	6.218483
6.138033	446.372278	6.223488
5.679394	450.149029	6.228493
5.719072	451.816514	6.233498
5.501028	448.927315	6.238502
5.187290	445.856951	6.243507
5.829918	447.455274	6.248512
5.332956	447.431925	6.253517
5.515303	442.211516	6.258522
5.622702	462.035186	6.263526
5.971329	455.909170	6.268531
5.806207	448.857551	6.273536
5.336976	451.936752	6.278541
5.729588	451.799332	6.283546
5.843033	462.320355	6.288550
6.138670	450.836761	6.293555
5.919196	448.659650	6.298560
5.598592	449.668557	6.303565
5.712125	441.564013	6.308570
5.748917	447.072856	6.313574
5.569112	452.226484	6.318579
5.825656	446.848911	6.323584
5.356601	448.289214	6.328589
5.665698	450.642169	6.333594
5.869389	455.292773	6.338598
5.760757	450.889931	6.343603
5.624112	448.883346	6.348608
5.621103	450.760005	6.353613
5.618003	450.029671	6.358618
5.567281	450.796970	6.363622
5.883067	464.658948	6.368627
5.863275	450.117880	6.373632
5.645935	450.968234	6.378637
6.001079	446.179507	6.383642
5.824331	450.794803	6.388646
5.949164	448.623858	6.393651
5.891496	447.193373	6.398656
5.532655	453.669066	6.403661
5.718899	451.596070	6.408666
6.044635	452.421446	6.413670
5.830828	446.848642	6.418675
5.747665	447.070515	6.423680
5.540133	455.120242	6.428685
5.706373	446.931505	6.433690
5.791648	443.001334	6.438694
5.579453	452.225576	6.443699
5.959355	439.966300	6.448704
5.423157	447.836560	6.453709
5.817840	442.269661	6.458714
5.699826	444.831910	6.463718
5.593035	447.474661	6.468723
5.944132	442.626455	6.473728
5.815321	453.482831	6.478733
6.004799	443.012487	6.483738
5.735130	446.193301	6.488742
6.026596	443.050259	6.493747
5.656565	448.521601	6.498752
5.501140	448.033440	6.503757
5.871481	445.029904	6.508762
5.965226	446.682589	6.513766
5.691844	446.564096	6.518771
6.022488	444.224860	6.523776
5.922005	443.902101	6.528781
5.645761	442.214790	6.533786
5.554388	444.481792	6.538790
5.661592	445.604007	6.543795
5.586328	445.685432	6.548800
5.736336	446.364330	6.553805
6.392009	436.463205	6.558810
6.078626	442.548946	6.563814
5.769428	421.817314	6.568819
5.568127	411.398725	6.573824
5.351968	424.689105	6.578829
5.616819	414.494878	6.583834
5.825544	422.162985	6.588838
5.352663	429.754390	6.593843
5.965804	434.979930	6.598848
5.607449	443.271588	6.603853
5.662415	436.030461	6.608858
5.571905	444.938232	6.613862
5.318893	436.258353	6.618867
5.499629	445.199557	6.623872
5.409814	448.428123	6.628877
5.661479	439.292671	6.633882
5.835370	445.406472	6.638886
5.903650	445.860887	6.643891
6.032195	444.632187	6.648896
5.745349	449.774112	6.653901
6.152211	444.306547	6.658906
6.017607	449.370832	6.663910
5.787379	441.029076	6.668915
5.875112	424.889261	6.673920
5.758598	429.384379	6.678925
5.610239	419.055569	6.683930
6.064314	415.482083	6.688934
5.839797	423.392084	6.693939
5.904196	410.372319	6.698944
5.758890	426.973629	6.703949
5.637764	424.603937	6.708954
5.497392	422.971271	6.713958
5.665566	416.493883	6.718963
5.896833	424.987385	6.723968
5.551858	426.253216	6.728973
5.579699	415.127989	6.733978
5.624625	419.170691	6.738982
5.806230	422.730058	6.743987
6.005920	421.224450	6.748992
5.720500	419.652477	6.753997
5.910331	416.196325	6.759002
5.869651	420.907356	6.764006
5.662208	420.626667	6.769011
6.100998	418.662805	6.774016
5.684996	424.903828	6.779021
5.780568	429.125264	6.784026
5.784993	422.784264	6.789030
5.739524	423.557066	6.794035
6.017737	426.756439	6.799040
5.590890	433.021311	6.804045
5.547823	418.692729	6.809050
5.863010	423.455572	6.814054
5.870918	426.450517	6.819059
5.874819	420.299431	6.824064
5.431682	421.817930	6.829069
6.012637	424.700941	6.834074
5.482608	421.518934	6.839078
5.413017	425.272689	6.844083
5.427092	420.869611	6.849088
5.196921	423.142538	6.854093
5.889437	423.214399	6.859098
5.524347	421.164515	6.864102
5.684993	424.379144	6.869107
5.626713	415.807973	6.874112
5.296101	426.964878	6.879117
5.753498	424.896857	6.884122
5.733716	428.142921	6.889126
5.568785	433.151841	6.894131
5.965703	429.122222	6.899136
5.726260	431.273213	6.904141
5.793973	421.707836	6.909146
5.980353	417.002508	6.914150
5.928790	423.958406	6.919155
6.054416	421.917057	6.924160
5.664410	414.350179	6.929165
5.703298	414.809198	6.934170
5.949675	420.541465	6.939174
5.256944	419.909695	6.944179
5.651371	418.715269	6.949184
5.879934	414.810111	6.954189
5.500158	414.673486	6.959194
5.561549	418.609202	6.964198
5.424050	420.883427	6.969203
5.827331	418.286034	6.974208
5.400509	422.570335	6.979213
5.528902	424.432731	6.984218
5.998678	436.223556	6.989222
5.672943	428.830104	6.994227
6.123966	424.924890	6.999232
5.858908	415.879904	7.004237
5.753151	417.310738	7.009242
5.887866	423.905246	7.014246
5.686426	418.270402	7.019251
5.861197	415.117174	7.024256
5.878739	415.149256	7.029261
5.973033	420.209307	7.034266
5.923048	411.994352	7.039270
5.751702	423.613532	7.044275
5.659815	417.898245	7.049280
5.656400	425.735638	7.054285
5.441675	416.423330	7.059290
5.704711	416.938981	7.064294
5.811824	423.604254	7.069299
5.941561	424.710282	7.074304
5.744038	424.969055	7.079309
5.798952	423.840481	7.084314
5.945873	424.257263	7.089318
5.379395	425.972263	7.094323
5.769029	417.631475	7.099328
5.645995	425.728062	7.104333
5.511127	416.735445	7.109338
5.834356	418.070590	7.114342
5.662299	422.099833	7.119347
5.621943	423.802002	7.124352
5.894608	425.439308	7.129357
5.682005	415.313561	7.134362
5.696683	418.930721	7.139366
5.409340	418.630913	7.144371
5.730773	414.331543	7.149376
5.384279	424.431050	7.154381
5.834459	413.628801	7.159386
5.987772	418.211357	7.164390
5.477665	418.734248	7.169395
5.855416	412.708091	7.174400
5.144605	422.279368	7.179405
5.826816	407.995348	7.184410
5.938742	423.698950	7.189414
5.360433	412.393445	7.194419
5.491496	415.780391	7.199424
5.571877	423.996970	7.204429
5.505723	418.945221	7.209434
5.913834	425.351356	7.214438
5.760600	430.564092	7.219443
5.729443	421.805166	7.224448
5.635469	428.631665	7.229453
5.683429	427.035931	7.234458
5.683070	422.970482	7.239462
5.461308	432.879602	7.244467
5.983748	434.588507	7.249472
5.945096	443.181260	7.254477
5.690347	436.472727	7.259482
5.590369	426.130006	7.264486
5.147499	429.262022	7.269491
5.555083	437.148922	7.274496
5.579037	449.670851	7.279501
6.000003	442.381867	7.284506
5.934425	452.696809	7.289510
5.729233	443.838587	7.294515
5.868861	446.398434	7.299520
5.863174	451.701956	7.304525
5.785942	442.848996	7.309530
5.598011	432.719373	7.314534
5.685255	425.065058	7.319539
5.984587	430.001234	7.324544
5.628808	432.069210	7.329549
5.567251	426.833236	7.334554
5.691605	430.980558	7.339558
5.760110	441.068835	7.344563
6.347063	446.330120	7.349568
5.820309	437.025561	7.354573
5.693649	433.283628	7.359578
5.546068	424.400569	7.364582
5.640801	435.234564	7.369587
5.552102	423.143637	7.374592
5.369145	427.737752	7.379597
5.457293	426.426795	7.384602
5.988320	436.705199	7.389606
5.776464	444.176615	7.394611
5.757062	438.725219	7.399616
6.060467	428.866637	7.404621
5.736331	413.768991	7.409626
6.014116	419.967748	7.414630
5.327897	417.895411	7.419635
6.115706	405.866483	7.424640
5.633607	421.808695	7.429645
6.017597	415.104497	7.434650
6.281787	410.095907	7.439654
5.514930	420.204326	7.444659
5.842947	411.534664	7.449664
5.943264	417.419532	7.454669
5.710533	424.596811	7.459674
5.812265	420.787456	7.464678
5.520119	421.513484	7.469683
5.655710	417.774757	7.474688
5.450294	429.317019	7.479693
5.490726	421.110040	7.484698
5.962885	407.539157	7.489702
5.563451	409.177361	7.494707
5.824956	414.255505	7.499712
5.728953	413.770689	7.504717
5.828232	420.016398	7.509722
5.664179	414.473775	7.514726
5.638885	415.012456	7.519731
6.057220	405.047292	7.524736
5.629005	416.409313	7.529741
5.813258	411.666354	7.534746
5.840056	413.566814	7.539750
5.443127	411.911071	7.544755
5.641357	409.462868	7.549760
5.678305	419.166926	7.554765
5.741310	410.649523	7.559770
5.866113	413.471123	7.564774
5.797675	417.063339	7.569779
5.893009	414.466738	7.574784
5.374792	414.048076	7.579789
5.208979	414.387305	7.584794
5.765163	411.462226	7.589798
5.525642	429.002140	7.594803
5.564784	415.438985	7.599808
5.818755	422.714015	7.604813
5.787991	417.675705	7.609818
5.859555	415.636500	7.614822
5.663259	419.663213	7.619827
5.903823	421.147356	7.624832
5.604599	419.938223	7.629837
5.708891	417.874908	7.634842
6.095202	415.966726	7.639846
5.862732	422.406788	7.644851
5.876779	412.482819	7.649856
5.588228	416.315172	7.654861
5.830128	420.488368	7.659866
6.489333	413.177886	7.664870
5.833606	422.411494	7.669875
5.950226	416.929301	7.674880
5.574910	409.803060	7.679885
5.254012	420.195954	7.684890
5.338932	416.974545	7.689894
5.769119	418.913043	7.694899
5.834483	412.758657	7.699904
5.453465	419.396004	7.704909
5.768082	407.491838	7.709914
5.447906	419.014108	7.714918
5.716912	414.238885	7.719923
5.695445	413.774029	7.724928
5.511243	427.078387	7.729933
5.579493	421.157670	7.734938
5.599828	417.319940	7.739942
5.165958	424.332575	7.744947
5.833924	425.237209	7.749952
5.532730	425.610305	7.754957
5.748945	417.654203	7.759962
5.952213	427.227799	7.764966
5.502443	411.548710	7.769971
5.910113	420.767564	7.774976
5.531381	425.408173	7.779981
5.543154	428.396186	7.784986
5.866436	427.051551	7.789990
5.381325	424.134596	7.794995
5.891041	420.185385	7.800000
5.848791	432.540500	7.805005
5.796775	423.240661	7.810010
5.644087	419.853995	7.815014
5.558937	430.697188	7.820019
5.792509	422.567517	7.825024
5.475989	422.914540	7.830029
5.801358	436.487086	7.835034
5.900834	427.967124	7.840038
5.553046	426.493510	7.845043
5.737562	421.440451	7.850048
5.757006	427.322174	7.855053
5.393942	424.439882	7.860058
5.932501	437.672133	7.865062
5.798218	432.871507	7.870067
5.781829	429.545743	7.875072
5.628201	433.186112	7.880077
5.990478	436.441920	7.885082
5.639086	434.026046	7.890086
5.503603	432.269223	7.895091
5.763477	428.381304	7.900096
5.499777	430.779711	7.905101
5.738066	444.963873	7.910106
5.937762	442.373063	7.915110
5.404399	440.283101	7.920115
5.955029	445.464653	7.925120
5.881905	446.630942	7.930125
5.662201	439.337934	7.935130
5.875705	423.074007	7.940134
5.352937	432.486400	7.945152
5.688175	432.758947	7.950170
5.624003	450.627541	7.955187
5.617128	452.973387	7.960205
6.009782	443.476132	7.965222
5.650410	446.625126	7.970240
6.037095	442.219069	7.975258
5.658188	435.862783	7.980275
5.789352	429.814740	7.985293
5.725658	419.767313	7.990310
5.787015	424.519782	7.995328
5.732270	414.120667	8.000346
5.848871	427.568088	8.005363
5.481588	424.927481	8.010381
6.121369	431.934059	8.015398
5.725932	424.617858	8.020416
6.016067	425.440263	8.025434
5.736362	428.665132	8.030451
5.868828	419.584194	8.035469
5.839473	412.541994	8.040486
5.769531	419.697638	8.045504
6.150904	414.146877	8.050522
6.211846	416.519961	8.055539
5.701657	423.018759	8.060557
5.969270	418.602963	8.065574
5.773521	421.887259	8.070592
6.169484	412.190689	8.075610
6.021140	419.093533	8.080627
5.893138	416.980318	8.085645
5.557852	419.885695	8.090662
5.837596	416.241161	8.095680
5.943502	412.993091	8.100698
5.381782	412.143869	8.105715
5.508180	420.976020	8.110733
6.082608	417.894377	8.115750
5.546977	420.073760	8.120768
6.012946	432.772176	8.125786
5.713914	425.223121	8.130803
5.919929	439.795774	8.135821
6.039421	441.471729	8.140838
6.034286	449.324124	8.145856
6.051369	443.981909	8.150874
5.862359	422.874204	8.155891
5.530884	429.499635	8.160909
5.975652	437.313090	8.165926
6.133070	449.154156	8.170944
5.903778	448.483218	8.175962
6.294045	447.399628	8.180979
5.825372	425.215439	8.185997
6.202009	427.640045	8.191014
5.732104	425.895977	8.196032
5.926150	417.117813	8.201050
5.724732	439.870939	8.206067
6.007475	452.055284	8.211085
6.275303	446.781077	8.216102
6.284049	452.763081	8.221120
6.153395	433.486036	8.226138
5.794809	427.571533	8.231155
5.811377	422.617564	8.236173
6.104952	421.268262	8.241190
5.973002	440.103664	8.246208
6.012038	445.418208	8.251226
5.984221	450.919951	8.256243
5.781389	451.036966	8.261261
6.158852	444.319172	8.266278
5.959100	453.896711	8.271296
5.881086	451.305450	8.276314
5.319658	449.231741	8.281331
5.663105	449.777554	8.286349
5.877770	449.403124	8.291366
5.886798	451.825372	8.296384
5.731507	447.800875	8.301402
6.276223	455.358839	8.306419
6.060468	452.006528	8.311437
6.041240	444.180097	8.316454
5.859910	449.652244	8.321472
5.949999	462.845072	8.326490
6.166930	466.071027	8.331507
6.112349	477.598194	8.336525
6.556484	464.425849	8.341542
6.229416	458.168729	8.346560
6.011886	449.808483	8.351578
5.881634	452.836372	8.356595
5.750120	460.314101	8.361613
6.163598	469.511546	8.366630
5.902442	475.008832	8.371648
6.018577	480.617416	8.376666
6.284069	472.525457	8.381683
6.277988	475.423442	8.386701
6.462958	474.315213	8.391718
6.368470	470.650410	8.396736
6.159373	474.309189	8.401754
6.599711	477.932483	8.406771
6.201128	474.122824	8.411789
6.456716	458.237655	8.416806
6.358969	454.671195	8.421824
6.035666	456.934078	8.426842
6.104922	446.957323	8.431859
6.266134	454.635335	8.436877
6.119208	453.566486	8.441894
6.516298	460.447001	8.446912
6.153825	449.038896	8.451930
6.092260	443.292442	8.456947
6.210539	463.442488	8.461965
6.386944	462.774255	8.466982
6.048893	457.727518	8.472000
6.509998	465.393259	8.477018
6.304336	464.750176	8.482035
5.993320	458.272793	8.487053
6.662184	459.114754	8.492070
6.384292	455.715373	8.497088
6.077953	449.085784	8.502106
6.258670	459.048677	8.507123
6.024265	470.102245	8.512141
6.104001	471.689759	8.517158
6.673153	473.386781	8.522176
6.519339	479.886566	8.527194
6.923959	464.650221	8.532211
6.309373	461.256258	8.537229
6.351507	447.108662	8.542246
6.290611	445.373090	8.547264
6.354788	447.909771	8.552282
6.284260	451.531055	8.557299
6.122764	449.643989	8.562317
6.468903	452.082844	8.567335
6.556467	449.355188	8.572352
6.358153	448.780380	8.577370
6.472956	442.930554	8.582387
6.078344	447.871236	8.587405
6.542521	457.095444	8.592423
6.466863	463.914334	8.597440
6.327470	467.035174	8.602458
6.800973	465.313698	8.607475
6.166630	456.072024	8.612493
5.950278	456.481488	8.617511
6.359655	469.602204	8.622528
6.173470	470.445595	8.627546
6.455948	476.955913	8.632563
6.129479	479.986148	8.637581
6.469777	480.197943	8.642599
6.329952	477.764685	8.647616
6.209816	483.243033	8.652634
6.599757	473.395897	8.657651
6.291995	474.532890	8.662669
6.348948	480.390586	8.667687
6.678980	475.242322	8.672704
6.286746	473.927889	8.677722
6.491399	474.751067	8.682739
6.175426	476.047136	8.687757
6.653270	475.697741	8.692775
6.323839	470.100545	8.697792
6.190680	475.306379	8.702810
6.553622	488.216635	8.707827
6.696303	489.305143	8.712845
6.442522	491.607629	8.717863
6.639831	480.799756	8.722880
6.658197	482.090776	8.727898
6.584054	475.396393	8.732915
6.461772	473.181291	8.737933
6.610416	479.677866	8.742951
6.895681	483.824072	8.747968
6.421195	477.757300	8.752986
6.504549	470.397619	8.758003
6.319167	476.697223	8.763021
6.904020	491.500892	8.768039
6.581084	485.110573	8.773056
6.449692	488.062907	8.778074
6.692045	501.216128	8.783091
6.711275	501.850611	8.788109
6.593039	490.902826	8.793127
6.634702	494.175182	8.798144
6.678616	499.577340	8.803162
7.072294	488.464141	8.808179
6.859506	487.307781	8.813197
6.419899	487.231523	8.818215
6.530925	476.096347	8.823232
6.681636	470.326091	8.828250
6.567256	478.198771	8.833267
6.311334	497.621698	8.838285
6.306772	497.480431	8.843303
6.571968	505.602916	8.848320
6.632140	508.231752	8.853338
6.689860	501.857523	8.858355
6.835330	505.498622	8.863373
6.588966	505.376307	8.868391
6.938217	507.155123	8.873408
6.501018	508.896219	8.878426
6.945313	506.532379	8.883443
7.061697	508.218295	8.888461
6.869010	508.371590	8.893479
7.228002	507.573762	8.898496
7.048185	508.305704	8.903514
6.958045	490.593830	8.908531
6.716677	491.392220	8.913549
6.502903	487.929139	8.918567
6.956317	495.144822	8.923584
6.622715	503.667239	8.928602
6.696211	500.616734	8.933619
6.592006	509.538708	8.938637
6.686421	500.599390	8.943655
6.987877	503.177796	8.948672
6.826583	505.806618	8.953690
7.066452	504.885444	8.958707
6.793675	503.025275	8.963725
6.761688	505.952570	8.968743
7.029335	501.470477	8.973760
6.583133	507.520626	8.978778
6.942878	507.356992	8.983795
6.514795	511.192100	8.988813
6.497106	504.138568	8.993831
6.759529	495.125592	8.998848
6.708404	507.015150	9.003866
6.813503	501.315147	9.008883
6.867618	506.428532	9.013901
6.849701	497.478413	9.018919
7.088301	504.872924	9.023936
6.521108	507.688419	9.028954
6.769197	502.950616	9.033971
6.808879	511.039010	9.038989
7.128276	505.980766	9.044007
6.780081	502.390423	9.049024
6.827285	508.274902	9.054042
6.925716	496.652540	9.059059
7.248621	501.269376	9.064077
6.927216	511.500320	9.069095
6.986935	510.115069	9.074112
6.865131	517.856387	9.079130
7.182161	499.130816	9.084147
7.090422	508.154978	9.089165
6.687003	504.387095	9.094183
6.884614	501.320298	9.099200
6.940891	521.795703	9.104218
7.464316	519.517293	9.109235
7.362053	511.072686	9.114253
6.837638	511.782882	9.119271
6.756037	499.459741	9.124288
6.873003	514.106367	9.129306
7.199069	526.094628	9.134323
6.928821	523.454582	9.139341
7.055668	530.106068	9.144359
7.321088	525.157261	9.149376
7.009527	515.060256	9.154394
6.998834	522.900931	9.159411
6.977461	527.925164	9.164429
6.946390	524.954155	9.169447
7.281585	532.806910	9.174464
7.471480	527.841534	9.179482
7.389712	518.207136	9.184499
7.089807	510.901177	9.189517
6.849118	509.913288	9.194535
7.178364	508.479496	9.199552
6.903126	523.736688	9.204570
6.871453	527.320341	9.209587
7.049426	534.001688	9.214605
7.235038	523.265049	9.219623
7.357723	528.399254	9.224640
7.382453	536.436355	9.229658
7.375095	526.695621	9.234675
7.552649	530.792443	9.239693
6.658134	519.571796	9.244711
7.386114	528.432818	9.249728
7.209647	541.295086	9.254746
7.163614	529.518615	9.259763
7.399682	541.334796	9.264781
7.109871	537.593286	9.269799
7.402635	528.455619	9.274816
7.100748	528.752256	9.279834
6.943563	534.290073	9.284851
7.465327	531.910936	9.289869
7.257571	534.168347	9.294887
7.727702	531.491189	9.299904
7.509908	527.293432	9.304922
7.394189	512.166978	9.309939
7.189662	500.907660	9.314957
7.139334	509.704430	9.319975
7.161300	509.145599	9.324992
7.116327	517.717472	9.330010
7.433420	523.685901	9.335027
7.479541	524.890525	9.340045
7.147026	523.532017	9.345063
7.214006	523.243841	9.350080
7.053231	530.827170	9.355098
7.471479	520.647370	9.360115
7.547842	528.127271	9.365133
7.283377	537.456219	9.370151
7.372530	527.274332	9.375168
7.235252	534.295406	9.380186
7.484941	524.646940	9.385203
7.715533	531.796566	9.390221
7.233523	542.699628	9.395239
7.512550	534.289941	9.400256
7.596532	531.452381	9.405274
7.486045	521.481657	9.410291
7.412103	517.592720	9.415309
7.263900	518.218725	9.420327
7.170059	528.022705	9.425344
7.548141	528.632521	9.430362
7.461856	532.739125	9.435379
7.454328	527.403897	9.440397
7.282379	537.434714	9.445415
7.284136	531.290148	9.450432
7.281327	529.141526	9.455450
7.171476	529.881441	9.460467
7.651247	525.470247	9.465485
7.355945	538.916018	9.470503
7.392514	527.767230	9.475520
7.640500	527.731560	9.480538
7.603932	524.414275	9.485555
7.657998	527.915066	9.490573
7.217491	535.624277	9.495591
7.441844	538.132718	9.500608
7.616534	538.970062	9.505626
7.600646	537.088574	9.510643
7.648629	530.930454	9.515661
7.550518	544.351645	9.520679
7.598745	528.076028	9.525696
7.369543	534.925314	9.530714
7.442726	530.148637	9.535731
7.489590	534.360611	9.540749
7.133492	530.954535	9.545767
7.211118	537.405454	9.550784
7.438273	547.575714	9.555802
7.321912	551.279938	9.560819
7.625359	560.576721	9.565837
7.434965	559.350576	9.570855
7.429300	560.774754	9.575872
7.360084	560.059796	9.580890
7.652298	558.013267	9.585907
7.414153	561.136974	9.590925
7.531752	563.390747	9.595943
7.562792	562.230892	9.600960
7.545079	573.200080	9.605978
7.576746	565.009017	9.610995
7.849817	562.091332	9.616013
7.708423	572.638087	9.621031
7.623061	562.060647	9.626048
7.563196	567.463306	9.631066
7.447482	562.810891	9.636083
8.004591	573.409148	9.641101
7.541019	571.828174	9.646119
7.927780	568.132128	9.651136
7.649038	563.006641	9.656154
7.320037	569.600179	9.661171
7.814531	573.830388	9.666189
7.719789	593.139802	9.671207
8.097111	596.126056	9.676224
7.807250	594.407410	9.681242
7.646189	585.230368	9.686259
7.480558	580.484783	9.691277
7.512971	594.125401	9.696295
7.507770	587.988217	9.701312
7.896245	595.201493	9.706330
7.683921	595.468318	9.711347
8.082847	582.208296	9.716365
7.637014	587.516802	9.721383
7.697170	590.820993	9.726400
7.713957	587.997108	9.731418
7.720937	598.580591	9.736435
8.051533	597.017192	9.741453
7.842124	590.814174	9.746471
7.927007	593.022585	9.751488
8.115626	587.400986	9.756506
8.098448	598.155511	9.761523
7.786436	593.663232	9.766541
7.763080	597.302400	9.771559
7.898730	590.843346	9.776576
8.249380	589.403038	9.781594
7.874953	594.406869	9.786611
8.132820	579.316497	9.791629
7.871913	583.882817	9.796647
8.031979	586.581219	9.801664
7.810667	578.505527	9.806682
7.722129	592.253456	9.811699
8.210957	591.340607	9.816717
7.962542	586.544876	9.821735
7.988465	591.552250	9.826752
8.038536	589.777186	9.831770
8.265019	587.598942	9.836787
8.304781	580.337564	9.841805
8.113841	588.121302	9.846823
8.303188	593.453364	9.851840
8.667338	589.407408	9.856858
8.200754	578.012377	9.861875
7.925788	569.613737	9.866893
7.833584	581.490846	9.871911
8.158866	580.928670	9.876928
8.270349	586.427563	9.881946
8.232523	595.897757	9.886963
8.369800	582.120154	9.891981
8.070252	571.743525	9.896999
7.815618	564.834392	9.902016
8.133301	576.044519	9.907034
7.910739	580.740530	9.912051
8.595244	579.200576	9.917069
8.396559	571.446389	9.922087
8.152830	568.615989	9.927104
7.957433	563.275472	9.932122
8.029775	564.889399	9.937139
7.742464	564.489478	9.942157
7.965162	578.441095	9.947175
8.156315	578.663636	9.952192
8.562815	578.716738	9.957210
8.159683	595.123804	9.962227
8.277318	578.048318	9.967245
8.350782	586.191413	9.972263
8.054902	583.457544	9.977280
8.389522	587.756988	9.982298
8.313276	590.186304	9.987315
8.356447	583.596575	9.992333
7.887954	581.369433	9.997351
8.135734	586.881685	10.002368
8.439757	589.251419	10.007386
8.001282	587.546591	10.012403
8.257691	585.215336	10.017421
8.422675	586.208837	10.022439
8.284275	581.777721	10.027456
8.767319	583.664970	10.032474
8.528508	586.832967	10.037491
8.162752	579.843410	10.042509
8.414551	583.310075	10.047527
8.517743	576.291224	10.052544
8.263976	564.436825	10.057562
7.892241	573.258738	10.062579
8.261106	571.547335	10.067597
8.280215	575.419686	10.072615
8.215382	588.832540	10.077632
8.024619	596.262805	10.082650
8.094478	582.729295	10.087667
8.310464	594.696980	10.092685
8.523187	587.515796	10.097703
8.327763	581.799738	10.102720
8.535991	580.182931	10.107738
8.453425	584.554051	10.112755
8.553321	586.693837	10.117773
8.500795	577.846931	10.122791
8.334540	596.173477	10.127808
8.432689	587.044183	10.132826
8.454281	597.076266	10.137843
8.348553	584.434955	10.142861
8.249986	585.286714	10.147879
8.323379	591.646798	10.152896
8.652137	580.496378	10.157914
7.881652	595.525115	10.162931
8.220891	587.377369	10.167949
8.635717	598.808974	10.172967
8.676132	609.071645	10.177984
8.591638	590.765496	10.183002
8.515826	596.391568	10.188019
8.500665	593.698920	10.193037
8.543594	596.365184	10.198055
8.123117	613.226264	10.203072
8.614994	611.568167	10.208090
8.541275	617.503187	10.213107
8.778471	618.507465	10.218125
8.692555	617.596305	10.223143
8.486809	618.187148	10.228160
8.962539	615.442829	10.233178
8.668727	616.703877	10.238195
8.692466	611.957015	10.243213
9.154365	610.559235	10.248231
8.700644	605.745174	10.253248
8.554217	586.984830	10.258266
8.580520	590.805564	10.263283
8.550702	584.258830	10.268301
8.524777	595.175669	10.273319
8.712167	603.995198	10.278336
8.973463	600.665942	10.283354
8.577630	587.495728	10.288371
8.634690	592.927412	10.293389
8.833962	594.887527	10.298407
8.406292	595.320637	10.303424
8.903351	599.133885	10.308442
8.771619	617.101594	10.313459
8.587672	622.025094	10.318477
9.122577	615.626551	10.323495
8.956480	609.243171	10.328512
8.674339	588.443351	10.333530
8.744354	590.003997	10.338547
8.795642	592.429110	10.343565
8.698387	585.520556	10.348583
8.516745	596.105189	10.353600
8.773265	599.975061	10.358618
8.725793	615.682637	10.363635
8.998265	619.316484	10.368653
9.264992	609.406528	10.373671
9.024596	608.469080	10.378688
9.087734	587.406879	10.383706
8.765257	585.011692	10.388723
8.987133	586.059394	10.393741
9.055709	580.011639	10.398759
8.812022	583.088881	10.403776
8.758027	582.743921	10.408794
8.763236	581.035848	10.413811
8.358471	579.524554	10.418829
8.542455	595.369416	10.423847
8.682407	611.334800	10.428864
8.883432	603.369648	10.433882
9.262502	605.434136	10.438899
8.803642	603.836642	10.443917
9.069359	607.499947	10.448935
8.981141	615.043540	10.453952
8.991723	607.726763	10.458970
8.739951	613.064830	10.463987
8.980247	610.650890	10.469005
9.253751	605.161153	10.474023
8.877571	617.947470	10.479040
8.979120	610.790007	10.484058
8.952194	610.655400	10.489075
9.062876	612.837680	10.494093
9.112274	612.621686	10.499111
8.897500	614.577249	10.504128
8.975467	606.653467	10.509146
9.303673	614.583094	10.514163
8.967746	615.976972	10.519181
9.208689	614.837874	10.524199
8.922466	611.190461	10.529216
8.778458	613.267480	10.534234
8.964162	607.699980	10.539251
8.825317	607.153719	10.544269
9.030361	599.282613	10.549287
9.029352	607.443699	10.554304
9.003420	608.744825	10.559322
9.103505	625.271889	10.564339
9.516181	623.462099	10.569357
9.391087	617.239549	10.574375
9.240031	617.364231	10.579392
8.860617	604.522791	10.584410
9.081547	613.879868	10.589427
9.087878	622.980240	10.594445
9.301691	621.750718	10.599463
9.303217	620.989959	10.604480
9.009513	625.028097	10.609498
9.257628	624.096158	10.614515
9.253800	637.038742	10.619533
9.474731	626.709918	10.624551
9.205445	631.340680	10.629568
8.877578	631.379456	10.634586
9.203871	633.505866	10.639603
9.318332	633.478493	10.644621
9.526949	636.648977	10.649639
9.302149	638.113808	10.654656
9.148656	629.418396	10.659674
9.367639	637.320965	10.664691
9.469069	637.677486	10.669709
9.511220	632.271326	10.674727
9.486710	633.083082	10.679744
9.527244	639.255827	10.684762
9.100580	621.624953	10.689779
9.418148	627.293540	10.694797
9.601982	628.034782	10.699815
9.588064	627.134431	10.704832
9.765697	618.024225	10.709850
9.383803	613.347230	10.714867
9.268335	610.982720	10.719885
9.451698	595.547403	10.724903
9.522291	600.232200	10.729920
8.991193	598.889021	10.734938
9.153390	601.391432	10.739955
9.193420	617.132636	10.744973
9.495834	618.656871	10.749991
9.273846	631.188665	10.755008
9.365430	633.048893	10.760026
9.276590	622.150069	10.765043
9.086762	628.564032	10.770061
9.538254	622.945416	10.775079
9.415475	631.564249	10.780096
9.713725	631.148317	10.785114
9.632414	624.663285	10.790131
9.719599	635.107990	10.795149
9.616487	631.996771	10.800167
9.829982	636.539267	10.805184
9.422178	631.045818	10.810202
9.585329	632.497200	10.815219
9.224713	638.546607	10.820237
9.680063	630.134495	10.825255
9.508063	629.350431	10.830272
9.393261	640.846113	10.835290
9.629986	622.682106	10.840307
9.322650	625.523175	10.845325
10.062511	633.965823	10.850343
9.634989	631.530283	10.855360
9.441694	630.967307	10.860378
9.870100	630.865497	10.865395
9.797123	640.880865	10.870413
9.493534	632.590821	10.875431
9.497019	630.049880	10.880448
9.376838	628.979987	10.885466
9.764444	643.716858	10.890483
9.898379	658.023272	10.895501
10.104976	663.952256	10.900519
9.547761	645.297240	10.905536
9.388330	645.480039	10.910554
9.593426	659.118896	10.915571
9.707788	666.564499	10.920589
9.879827	663.078803	10.925607
9.934291	663.859250	10.930624
9.678354	669.393647	10.935642
10.442228	657.203014	10.940659
10.235826	665.307945	10.945677
9.673858	644.387802	10.950695
9.787452	641.173200	10.955712
9.684231	638.065153	10.960730
9.807395	648.021390	10.965747
9.733129	662.540311	10.970765
9.917596	651.103185	10.975783
9.993211	663.932355	10.980800
10.084074	662.100400	10.985818
9.846026	662.456464	10.990835
9.966050	663.927229	10.995853
10.054809	657.103112	11.000871
10.077914	648.490474	11.005888
9.667477	645.477899	11.010906
9.765525	647.677942	11.015923
9.623801	659.736432	11.020941
9.752493	655.427551	11.025959
10.042258	656.789669	11.030976
9.742195	659.206726	11.035994
10.315181	653.042044	11.041011
10.084410	657.673089	11.046029
10.183310	658.598053	11.051047
10.120197	660.438340	11.056064
9.803758	660.942386	11.061082
9.706982	652.862926	11.066099
9.941901	670.407167	11.071117
10.074483	671.156440	11.076135
10.042284	663.808473	11.081152
9.879706	670.284453	11.086170
10.194814	660.120735	11.091187
9.835229	666.031134	11.096205
10.343387	670.764155	11.101223
10.089423	664.220953	11.106240
9.758278	670.385673	11.111258
9.953868	670.083656	11.116275
10.061882	671.824548	11.121293
10.028878	657.313017	11.126311
10.133821	667.120641	11.131328
9.994205	659.985167	11.136346
9.927835	661.276853	11.141363
10.153015	685.033270	11.146381
10.120099	694.098802	11.151399
10.698260	686.358545	11.156416
10.187224	679.764098	11.161434
10.337300	673.343779	11.166451
10.373120	678.030889	11.171469
10.263726	672.932485	11.176487
10.061720	668.179953	11.181504
9.999730	682.539176	11.186522
10.076761	689.968546	11.191539
9.995635	695.096863	11.196557
10.240685	687.244697	11.201575
10.252996	688.022283	11.206592
10.327081	698.349157	11.211610
10.041456	697.137923	11.216627
10.185095	695.032607	11.221645
10.491370	701.892731	11.226663
10.330585	693.441428	11.231680
10.422105	698.640526	11.236698
10.271931	691.222669	11.241715
10.381427	694.279306	11.246733
10.603940	694.910348	11.251751
10.228261	696.417759	11.256768
10.279190	698.918682	11.261786
10.523702	688.292637	11.266803
10.344971	698.400346	11.271821
10.553205	705.335793	11.276839
10.357207	693.702631	11.281856
10.425262	695.118425	11.286874
10.474416	679.984931	11.291891
10.398133	688.694336	11.296909
10.463876	684.035549	11.301927
10.541337	693.386744	11.306944
10.359570	701.222743	11.311962
10.951035	689.772316	11.316979
10.636289	690.740002	11.321997
10.338781	689.543254	11.327015
10.614842	691.781683	11.332032
10.662545	696.883504	11.337050
10.336983	691.878925	11.342067
10.520226	695.088110	11.347085
10.313896	697.698769	11.352103
10.213398	698.345707	11.357120
10.213913	716.725142	11.362138
10.448939	709.234300	11.367155
10.545418	711.791205	11.372173
10.902532	712.625221	11.377191
11.039013	717.132467	11.382208
10.772637	721.289422	11.387226
10.821685	718.564604	11.392243
10.656537	717.340803	11.397261
10.769961	721.529769	11.402279
10.930365	712.213931	11.407296
10.480639	708.819334	11.412314
10.588428	711.437583	11.417331
10.504619	723.001045	11.422349
10.610243	716.682350	11.427367
10.633375	715.719385	11.432384
10.406420	717.424403	11.437402
10.364318	719.826296	11.442419
10.605880	721.517865	11.447437
10.408058	717.168610	11.452455
10.798056	707.226662	11.457472
10.219857	721.761472	11.462490
10.630485	719.986707	11.467507
10.794199	733.367016	11.472525
11.034992	734.459101	11.477543
11.054401	730.243065	11.482560
10.670708	736.220380	11.487578
10.950153	732.976619	11.492595
11.038846	735.913446	11.497613
11.062404	732.384729	11.502631
11.223106	725.899610	11.507648
10.730010	730.925228	11.512666
10.870645	720.062973	11.517683
10.739496	728.089870	11.522701
10.894703	738.154746	11.527719
10.932149	732.742982	11.532736
10.911041	741.942388	11.537754
10.820048	736.847395	11.542771
10.764202	743.410821	11.547789
11.089078	739.175323	11.552807
11.078002	729.166816	11.557824
10.845493	745.190678	11.562842
10.779148	730.599105	11.567859
11.004034	726.271979	11.572877
11.010083	735.937345	11.577895
11.280466	733.483960	11.582912
11.019550	732.710667	11.587930
11.237365	734.822528	11.592947
11.050141	734.312245	11.597965
11.044188	737.595263	11.602983
11.165747	739.851595	11.608000
10.889895	741.346524	11.613018
10.831478	740.427893	11.618035
10.787192	742.489302	11.623053
10.777362	742.399352	11.628071
10.840167	739.123262	11.633088
11.140812	763.877823	11.638106
11.149268	759.313199	11.643123
11.343232	764.619342	11.648141
11.324745	767.721291	11.653159
11.277166	765.027385	11.658176
11.423234	760.204513	11.663194
11.424052	756.152331	11.668211
11.268715	739.371927	11.673229
11.053743	748.993034	11.678247
11.373013	746.983271	11.683264
11.325656	751.762328	11.688282
11.232398	755.046405	11.693299
11.470794	751.518737	11.698317
11.295970	753.597444	11.703335
11.479669	737.922109	11.708352
11.339278	749.024235	11.713370
11.271890	734.805209	11.718387
11.530689	732.839636	11.723405
11.252929	744.998394	11.728423
11.445689	729.817110	11.733440
11.282630	732.118035	11.738458
11.115493	745.783723	11.743475
11.752441	756.356957	11.748493
11.095568	751.271727	11.753511
11.437189	754.203642	11.758528
11.939536	762.222814	11.763546
11.884331	750.599114	11.768563
11.476549	739.488258	11.773581
11.256979	743.969246	11.778599
11.285624	738.186472	11.783616
10.886020	740.464500	11.788634
11.106994	756.158541	11.793651
11.397872	756.154020	11.798669
11.371547	759.310845	11.803687
11.627635	756.563049	11.808704
11.626207	764.705337	11.813722
11.222805	769.871547	11.818739
11.936990	758.638536	11.823757
11.455959	777.620506	11.828775
11.463088	772.071468	11.833792
11.447793	766.649022	11.838810
11.370137	766.333012	11.843827
11.578890	766.669565	11.848845
11.347493	771.695215	11.853863
11.676020	756.950232	11.858880
11.043298	774.390676	11.863898
11.525679	781.683989	11.868915
11.947340	782.457402	11.873933
11.958130	788.202510	11.878951
11.610269	778.148913	11.883968
11.939303	773.947471	11.888986
11.809824	777.988314	11.894003
12.015815	771.653875	11.899021
11.826895	764.690186	11.904039
12.039407	765.641536	11.909056
12.015014	768.359400	11.914074
11.939641	772.035156	11.919091
11.996175	766.538339	11.924109
11.745411	763.645893	11.929127
11.866051	769.667277	11.934144
11.665816	767.145613	11.939162
11.578936	764.735577	11.944179
11.952910	767.157492	11.949197
11.718932	776.273503	11.954215
11.868377	758.921459	11.959232
11.543149	773.145272	11.964250
11.728693	764.907917	11.969267
11.643433	765.890144	11.974285
11.758436	781.686019	11.979303
11.958596	787.868519	11.984320
12.318584	791.946285	11.989338
12.067811	783.509039	11.994355
12.077335	768.249134	11.999373
11.852665	776.723054	12.004391
11.757902	775.100054	12.009408
12.138183	770.474013	12.014426
11.946815	784.026761	12.019443
11.952836	785.830982	12.024461
12.155947	799.164142	12.029479
12.157577	786.212374	12.034496
12.296748	776.568467	12.039514
11.832963	769.187092	12.044531
12.451720	765.432566	12.049549
12.207818	766.149313	12.054567
12.117040	760.407334	12.059584
11.861768	765.676567	12.064602
11.839835	763.685548	12.069619
11.989608	785.263768	12.074637
12.416249	797.905491	12.079655
12.192240	778.737375	12.084672
12.254372	773.810884	12.089690
11.827790	768.844203	12.094707
12.211867	781.233804	12.099725
12.245021	795.534028	12.104743
12.232390	793.557328	12.109760
12.342186	796.443520	12.114778
12.321192	801.562446	12.119795
12.421557	780.301680	12.124813
12.112027	775.752161	12.129831
11.692412	773.542582	12.134848
12.088154	792.346168	12.139866
12.114771	799.177562	12.144883
12.542733	793.556268	12.149901
12.421936	793.073446	12.154919
12.366456	796.765026	12.159936
12.483593	788.393210	12.164954
12.404034	789.099987	12.169971
12.776378	788.795521	12.174989
12.277717	801.519108	12.180007
12.335665	796.403916	12.185024
12.355926	792.194044	12.190042
12.074529	796.003072	12.195059
12.143412	796.620319	12.200077
11.859426	805.608480	12.205095
12.429771	794.467411	12.210112
12.398009	796.943435	12.215130
12.188681	798.270153	12.220147
12.085072	799.788593	12.225165
12.092319	807.913763	12.230183
12.177635	819.958878	12.235200
12.472844	815.361934	12.240218
12.234707	823.591831	12.245235
12.569710	820.721206	12.250253
12.609587	829.065337	12.255271
12.826848	825.869173	12.260288
12.567179	823.025450	12.265306
12.514459	830.184872	12.270323
12.489124	827.294965	12.275341
12.652885	834.379443	12.280359
12.774870	833.643982	12.285376
12.752518	829.712180	12.290394
12.833385	829.257721	12.295411
12.574483	824.450945	12.300429
12.613037	827.310435	12.305447
12.587821	824.183822	12.310464
12.498630	828.748546	12.315482
12.412040	833.246591	12.320499
12.531749	829.787997	12.325517
12.556866	825.069266	12.330535
12.522674	829.836814	12.335552
12.810370	830.422933	12.340570
12.540399	831.494066	12.345587
12.847607	826.437642	12.350605
12.623121	829.833813	12.355623
12.727167	822.180408	12.360640
12.624639	824.746419	12.365658
12.617897	851.862495	12.370675
13.124161	854.620304	12.375693
12.975220	847.940657	12.380711
12.729762	853.265183	12.385728
13.035463	839.454682	12.390746
13.095892	847.994420	12.395763
13.078597	832.662922	12.400781
12.904620	826.839282	12.405799
12.622446	831.771919	12.410816
12.881399	829.288754	12.415834
12.541372	845.932317	12.420851
12.985953	859.073051	12.425869
13.020452	860.626662	12.430887
13.118300	852.103202	12.435904
13.537290	848.594556	12.440922
13.146302	844.117744	12.445939
13.230245	832.162915	12.450957
12.745908	834.211232	12.455975
12.656308	836.598491	12.460992
13.027123	835.928186	12.466010
13.179364	853.214159	12.471027
13.244408	858.086088	12.476045
13.553085	854.803011	12.481063
12.729766	834.232867	12.486080
13.198092	830.912157	12.491098
12.904547	839.327470	12.496115
12.848914	843.110602	12.501133
13.026995	849.801518	12.506151
12.811855	847.345295	12.511168
13.066665	851.007204	12.516186
13.049371	859.426580	12.521203
12.784530	856.012454	12.526221
13.014831	860.546062	12.531239
12.855411	865.838176	12.536256
12.778828	864.016657	12.541274
12.994849	875.713122	12.546291
13.213815	884.300622	12.551309
13.435790	886.443407	12.556327
13.241037	889.430982	12.561344
13.321950	878.615860	12.566362
13.478962	884.647362	12.571379
13.531989	882.098623	12.576397
13.686522	880.035761	12.581415
13.454150	878.017740	12.586432
13.437777	887.377428	12.591450
13.395577	888.902032	12.596467
13.375298	871.620653	12.601485
13.203867	875.898469	12.606503
13.189504	886.371856	12.611520
13.282110	880.200312	12.616538
13.137730	882.801291	12.621555
13.690456	887.647311	12.626573
13.534398	895.416249	12.631591
13.262015	890.823010	12.636608
13.438974	879.427941	12.641626
13.274031	879.930346	12.646643
13.092814	888.801459	12.651661
13.200316	878.515510	12.656679
13.028461	890.061317	12.661696
13.291644	891.743203	12.666714
13.296532	905.012824	12.671731
13.457261	903.611717	12.676749
13.662200	912.864158	12.681767
13.365617	916.227459	12.686784
13.620989	903.362084	12.691802
13.592356	914.771856	12.696819
13.707009	911.156246	12.701837
13.564963	915.293765	12.706855
13.788359	907.318662	12.711872
13.856335	910.820505	12.716890
13.742153	914.010058	12.721907
13.542139	911.257961	12.726925
13.687442	909.467945	12.731943
13.439264	918.305382	12.736960
14.059906	906.294816	12.741978
13.827706	909.496547	12.746995
13.952027	910.938258	12.752013
14.106579	907.341644	12.757031
13.520759	920.836376	12.762048
13.683298	910.036848	12.767066
13.572381	915.255104	12.772083
13.584942	918.958139	12.777101
13.439801	913.451850	12.782119
13.540092	917.803868	12.787136
13.797889	934.110844	12.792154
13.789952	935.156705	12.797171
13.851451	943.481722	12.802189
14.356002	931.912214	12.807207
14.200214	938.923723	12.812224
14.175356	930.372113	12.817242
13.918600	927.692022	12.822259
13.952442	915.580884	12.827277
13.852390	916.186733	12.832295
13.766689	938.594153	12.837312
13.924703	936.631726	12.842330
14.367342	943.391681	12.847347
14.417927	945.299391	12.852365
14.305889	927.508462	12.857383
13.868680	919.819898	12.862400
14.023532	917.974735	12.867418
14.201467	914.046248	12.872435
14.148509	914.834070	12.877453
13.890472	919.422116	12.882471
14.466646	929.588403	12.887488
14.125979	926.321846	12.892506
14.140645	918.325792	12.897523
13.876825	918.430274	12.902541
14.192602	934.330528	12.907559
14.469761	943.584292	12.912576
14.458876	937.258527	12.917594
14.326657	931.371505	12.922611
14.018731	924.893467	12.927629
14.178842	926.654624	12.932647
14.240815	939.381987	12.937664
14.054956	937.419789	12.942682
14.629542	939.636723	12.947699
14.255578	932.133908	12.952717
14.506852	935.382971	12.957735
14.390974	944.960254	12.962752
14.359670	938.814416	12.967770
14.286273	940.893033	12.972787
14.527267	941.805216	12.977805
14.590433	937.809497	12.982823
14.301095	945.510975	12.987840
14.331895	942.905749	12.992858
14.647905	944.645637	12.997875
14.229865	943.982162	13.002893
14.469823	934.555911	13.007911
14.176353	941.961385	13.012928
14.119862	942.967517	13.017946
14.423400	933.701722	13.022963
14.516632	939.759015	13.027981
14.488177	945.892182	13.032999
14.627762	940.988224	13.038016
14.344602	945.962073	13.043034
14.876433	947.882744	13.048051
14.303708	947.164608	13.053069
14.389564	942.941267	13.058087
14.383917	945.612038	13.063104
14.500812	937.085554	13.068122
14.700503	935.009297	13.073139
14.199068	938.934884	13.078157
14.533613	953.891769	13.083175
14.654614	972.886917	13.088192
14.641553	963.853752	13.093210
14.589329	970.874293	13.098227
14.227203	974.576085	13.103245
14.724428	970.171516	13.108263
14.646388	968.908803	13.113280
14.674273	969.996391	13.118298
14.839149	972.713033	13.123315
14.408907	975.481894	13.128333
14.764590	969.347997	13.133351
14.772636	983.150522	13.138368
14.756990	976.288993	13.143386
14.678009	969.847652	13.148403
14.731369	974.765625	13.153421
15.014498	971.224594	13.158439
14.483088	980.532481	13.163456
14.610270	984.814029	13.168474
15.065946	994.604749	13.173491
15.198770	1005.149820	13.178509
15.065858	1002.144193	13.183527
14.927367	997.671962	13.188544
15.007075	998.467404	13.193562
15.408856	996.646661	13.198579
15.140285	986.350145	13.203597
14.770138	984.479934	13.208615
14.812185	989.554322	13.213632
14.798147	1002.801733	13.218650
14.721750	1002.532860	13.223667
14.616626	1004.723754	13.228685
14.958558	1004.480856	13.233703
14.884978	998.149114	13.238720
14.947155	992.278951	13.243738
15.018977	1000.715989	13.248755
15.118324	1001.820785	13.253773
15.105230	1001.198003	13.258791
14.966239	1010.993542	13.263808
15.197027	1028.040154	13.268826
15.474991	1022.205600	13.273843
15.473449	1030.789850	13.278861
15.396433	1006.722632	13.283879
15.237848	997.500807	13.288896
15.051137	1007.726708	13.293914
15.550895	1015.591763	13.298931
15.344566	1018.189845	13.303949
15.333019	1000.992182	13.308967
15.411181	1005.735861	13.313984
15.166602	999.882200	13.319002
15.419016	1008.770638	13.324019
15.360901	1026.288557	13.329037
15.880762	1020.485532	13.334055
15.294048	1017.995984	13.339072
14.983691	1011.455178	13.344090
15.543023	1020.005193	13.349107
15.682137	1023.533783	13.354125
15.624007	1015.189323	13.359143
15.563241	1006.984137	13.364160
15.350665	1015.440495	13.369178
15.583700	1010.234693	13.374195
15.482360	1023.259108	13.379213
15.502238	1028.378006	13.384231
15.628010	1030.343374	13.389248
15.567355	1028.762345	13.394266
15.762978	1025.837786	13.399283
15.771441	1022.330312	13.404301
15.375277	1017.283053	13.409319
15.596972	1019.347002	13.414336
15.714085	1027.290951	13.419354
15.955642	1023.443992	13.424371
15.900723	1013.599989	13.429389
15.371496	1002.274462	13.434407
15.698125	1009.740599	13.439424
15.610095	1016.902471	13.444442
15.730192	1018.878195	13.449459
15.382842	1028.760039	13.454477
15.456697	1027.139000	13.459495
15.571810	1026.669702	13.464512
15.569886	1024.464076	13.469530
15.569084	1027.074138	13.474547
15.447678	1028.232460	13.479565
15.831841	1026.341889	13.484583
15.781142	1027.744758	13.489600
15.835092	1027.202991	13.494618
16.134167	1022.160411	13.499635
15.589816	1033.591100	13.504653
15.273500	1040.037652	13.509671
15.732709	1051.112291	13.514688
15.841062	1052.180965	13.519706
15.824297	1062.964107	13.524723
15.777139	1057.713828	13.529741
15.940990	1058.846392	13.534759
16.107158	1058.340691	13.539776
15.612580	1065.449514	13.544794
15.938660	1050.477450	13.549811
15.535718	1054.062573	13.554829
15.711779	1054.527334	13.559847
16.269014	1068.774064	13.564864
15.997328	1076.258233	13.569882
16.206463	1074.344587	13.574899
15.761927	1083.440095	13.579917
16.332770	1084.594101	13.584935
16.411764	1084.679585	13.589952
16.543368	1092.315172	13.594970
16.397448	1070.814932	13.599987
16.252818	1063.853655	13.605005
16.266778	1055.128642	13.610023
16.077078	1049.717658	13.615040
16.386996	1068.784296	13.620058
16.590016	1066.259368	13.625075
16.040421	1060.144202	13.630093
16.160230	1060.128614	13.635111
16.386839	1076.762507	13.640128
16.370887	1082.496120	13.645146
16.477833	1085.095621	13.650163
16.122683	1082.970579	13.655181
16.738760	1061.063773	13.660199
16.615074	1068.063991	13.665216
16.206057	1060.045893	13.670234
16.570819	1061.651919	13.675251
16.680768	1057.390061	13.680269
16.645833	1057.865790	13.685287
16.466497	1051.411740	13.690304
16.294566	1056.039979	13.695322
16.718324	1043.653062	13.700339
16.602871	1044.674749	13.705357
16.450732	1043.101741	13.710375
16.669010	1049.006932	13.715392
16.325354	1049.357458	13.720410
16.344265	1055.981870	13.725427
16.495876	1073.463818	13.730445
16.461222	1071.664111	13.735463
16.764131	1066.658788	13.740480
16.745203	1073.850883	13.745498
17.135893	1075.175130	13.750515
16.889642	1071.590788	13.755533
16.836432	1062.178846	13.760551
16.731836	1048.334639	13.765568
16.663056	1050.163231	13.770586
16.414448	1054.929719	13.775603
16.410811	1064.281191	13.780621
16.541205	1068.133056	13.785639
16.564629	1066.586189	13.790656
16.593265	1074.089575	13.795674
16.636680	1075.572378	13.800691
16.626809	1073.424797	13.805709
17.046000	1071.670748	13.810727
17.134016	1069.119656	13.815744
16.637641	1068.048717	13.820762
16.651799	1066.203492	13.825779
16.577280	1064.103912	13.830797
17.285712	1065.485674	13.835815
17.229177	1065.507184	13.840832
16.788164	1071.831270	13.845850
17.284666	1063.750189	13.850867
16.789789	1069.953322	13.855885
16.801637	1060.316588	13.860903
16.928325	1062.379648	13.865920
16.898302	1084.914230	13.870938
17.109899	1088.990068	13.875955
16.920780	1094.611958	13.880973
17.029752	1092.732940	13.885991
17.391440	1093.642000	13.891008
17.277081	1089.263797	13.896026
17.465560	1094.640327	13.901043
17.229921	1083.953576	13.906061
17.486036	1090.367262	13.911079
17.299649	1079.398235	13.916096
17.345358	1081.215203	13.921114
17.171044	1074.132337	13.926131
17.003283	1076.626552	13.931149
17.111659	1069.947531	13.936167
17.378365	1075.292863	13.941184
17.221133	1091.393604	13.946202
17.708804	1085.570355	13.951219
17.438695	1071.067236	13.956237
17.232063	1067.205282	13.961255
17.237482	1071.281861	13.966272
17.191978	1085.834489	13.971290
17.559757	1091.466954	13.976307
17.629424	1088.167634	13.981325
17.333700	1094.721435	13.986343
17.436747	1093.351443	13.991360
17.526170	1100.611780	13.996378
17.514780	1097.650215	14.001395
17.299882	1101.332120	14.006413
17.262720	1092.138561	14.011431
17.122807	1098.850991	14.016448
17.198099	1100.991538	14.021466
17.108587	1089.076340	14.026483
17.698022	1101.415052	14.031501
17.554209	1100.307806	14.036519
17.490757	1096.401320	14.041536
17.765949	1100.183167	14.046554
17.395056	1097.227435	14.051571
17.756893	1107.897634	14.056589
17.646552	1119.235129	14.061607
17.906671	1121.495046	14.066624
17.628718	1119.468360	14.071642
17.624128	1118.528652	14.076659
18.103436	1118.305255	14.081677
17.966914	1120.374847	14.086695
17.900235	1107.730204	14.091712
17.669146	1107.201536	14.096730
17.613080	1099.437396	14.101747
17.938909	1110.009094	14.106765
18.076587	1118.981838	14.111783
17.858752	1105.426736	14.116800
17.840989	1108.790569	14.121818
17.646383	1111.475192	14.126835
17.833341	1114.545012	14.131853
17.811622	1117.047908	14.136871
18.020561	1116.813223	14.141888
17.770764	1122.242652	14.146906
18.100666	1126.596616	14.151923
18.102171	1117.532689	14.156941
18.076300	1131.548931	14.161959
18.043147	1122.253739	14.166976
18.127390	1124.254027	14.171994
17.938587	1111.694789	14.177011
18.159155	1109.173418	14.182029
17.750764	1114.018607	14.187047
17.605032	1119.744164	14.192064
17.860667	1126.262082	14.197082
17.761036	1121.531259	14.202099
17.746686	1131.550339	14.207117
17.801754	1146.320793	14.212135
18.030413	1148.800244	14.217152
18.083465	1151.553370	14.222170
18.373789	1160.382294	14.227187
18.413909	1148.127999	14.232205
18.126595	1145.137073	14.237223
18.208566	1145.689163	14.242240
18.109183	1149.447656	14.247258
18.338927	1147.619139	14.252275
18.438264	1152.599387	14.257293
17.896919	1156.935229	14.262311
18.348405	1144.736407	14.267328
18.404157	1150.222115	14.272346
18.402588	1171.912879	14.277363
18.897615	1164.649362	14.282381
18.456087	1164.507125	14.287399
18.581880	1156.591386	14.292416
18.356866	1156.109103	14.297434
18.358444	1158.882919	14.302451
18.603776	1164.824936	14.307469
18.791177	1177.494945	14.312487
18.659988	1168.256116	14.317504
18.712249	1158.253225	14.322522
18.655285	1164.697056	14.327539
18.571614	1158.000754	14.332557
18.556573	1174.325451	14.337575
18.941945	1168.530827	14.342592
18.750299	1170.643777	14.347610
18.681190	1163.071008	14.352627
18.653353	1168.607689	14.357645
18.635897	1170.074790	14.362663
19.037258	1170.608398	14.367680
18.940289	1179.595846	14.372698
18.672571	1161.163183	14.377715
18.841412	1165.586574	14.382733
18.641180	1178.879069	14.387751
18.898936	1176.238249	14.392768
18.900546	1170.601587	14.397786
18.724159	1173.867206	14.402803
18.660926	1172.731550	14.407821
18.803581	1176.673039	14.412839
18.967541	1175.236690	14.417856
18.837353	1177.264270	14.422874
18.703579	1172.554563	14.427891
18.973066	1167.421901	14.432909
18.513102	1172.265718	14.437927
18.921018	1166.536993	14.442944
18.778460	1172.546100	14.447962
18.637017	1180.820972	14.452979
18.939452	1185.756784	14.457997
18.942123	1203.464174	14.463015
18.822832	1193.753238	14.468032
19.280914	1206.885801	14.473050
19.123572	1209.936997	14.478067
19.027161	1193.412030	14.483085
19.113785	1202.635820	14.488103
19.062543	1199.986605	14.493120
19.385225	1204.875067	14.498138
19.265918	1203.328460	14.503155
19.314474	1195.601536	14.508173
19.726388	1198.784452	14.513191
19.561567	1200.101070	14.518208
19.676147	1205.839518	14.523226
18.888219	1199.389249	14.528243
19.251955	1202.201005	14.533261
19.341177	1199.807501	14.538279
19.150155	1202.598877	14.543296
19.619305	1206.861613	14.548314
19.553912	1210.901980	14.553331
19.703976	1203.023445	14.558349
19.371188	1208.374383	14.563367
19.415798	1195.699616	14.568384
19.679835	1202.752750	14.573402
19.302081	1202.382762	14.578419
19.601795	1197.999617	14.583437
19.282810	1205.491251	14.588455
19.120661	1207.883615	14.593472
19.761046	1209.282362	14.598490
19.489683	1223.387635	14.603507
19.761920	1222.600215	14.608525
19.625065	1231.754890	14.613543
19.383630	1222.596425	14.618560
19.692224	1227.203069	14.623578
19.361544	1236.255567	14.628595
19.761042	1232.172370	14.633613
19.483287	1237.877623	14.638631
19.749465	1233.373488	14.643648
19.788625	1229.671809	14.648666
19.709414	1227.323628	14.653683
19.942013	1225.352639	14.658701
19.887545	1228.513956	14.663719
20.048066	1225.399198	14.668736
19.874513	1223.637019	14.673754
19.651744	1226.363942	14.678771
20.096862	1221.345762	14.683789
19.896685	1225.539800	14.688807
20.038815	1226.038284	14.693824
20.142746	1220.335080	14.698842
20.024092	1235.243284	14.703859
20.261770	1224.397079	14.708877
19.956778	1221.875984	14.713895
19.798375	1222.554105	14.718912
20.074545	1224.388629	14.723930
19.589232	1238.410667	14.728947
20.144496	1241.214511	14.733965
20.175807	1251.286465	14.738983
20.222360	1255.482878	14.744000
20.515943	1252.236810	14.749018
20.550204	1252.556530	14.754035
20.315202	1237.593323	14.759053
20.218969	1229.699716	14.764071
19.759987	1229.364547	14.769088
20.445455	1236.468432	14.774106
20.192339	1249.387399	14.779123
20.531610	1248.706243	14.784141
20.317375	1257.904615	14.789159
20.175256	1259.823616	14.794176
20.483179	1254.861639	14.799194
20.320319	1250.115442	14.804211
20.484936	1248.224533	14.809229
20.401061	1254.347553	14.814247
20.151574	1257.226995	14.819264
20.139213	1250.857169	14.824282
20.141612	1253.056494	14.829299
20.462142	1251.125376	14.834317
20.302970	1256.124066	14.839335
20.287921	1250.635160	14.844352
20.865350	1253.410287	14.849370
20.403457	1251.617540	14.854387
20.711616	1244.471636	14.859405
20.895134	1247.576732	14.864423
20.524210	1245.312125	14.869440
20.378898	1245.915610	14.874458
20.875109	1281.231494	14.879475
21.066913	1268.836582	14.884493
20.954375	1255.034486	14.889511
20.429374	1249.565520	14.894528
20.890492	1259.415496	14.899546
20.878719	1264.921287	14.904563
20.623832	1259.555167	14.909581
21.128972	1273.377864	14.914599
20.928297	1268.078989	14.919616
21.246280	1266.321844	14.924634
20.706597	1254.265623	14.929651
20.964452	1250.147809	14.934669
21.014126	1250.884850	14.939687
20.779963	1245.581762	14.944704
21.427630	1263.241802	14.949722
21.049664	1266.927199	14.954739
21.234543	1253.618166	14.959757
20.775672	1246.207419	14.964775
21.279058	1249.202436	14.969792
21.147472	1247.600942	14.974810
21.060755	1245.285494	14.979827
21.251356	1246.637949	14.984845
21.282467	1251.546861	14.989863
20.957869	1256.347400	14.994880
21.065692	1264.261351	14.999898
21.131161	1278.774656	15.004915
21.351028	1268.887458	15.009933
21.207882	1269.436954	15.014951
21.001886	1276.920381	15.019968
21.338678	1276.706688	15.024986
21.201642	1278.088389	15.030003
21.327658	1273.584113	15.035021
21.065198	1273.303360	15.040039
21.358215	1281.248265	15.045056
21.597992	1275.839351	15.050074
21.454914	1278.178242	15.055091
21.451039	1269.601091	15.060109
21.426370	1269.229431	15.065127
21.610453	1273.132890	15.070144
21.402334	1272.023085	15.075162
21.178552	1272.064488	15.080179
21.499233	1274.971367	15.085197
21.419154	1274.999722	15.090215
21.314372	1267.725998	15.095232
21.619183	1277.120775	15.100250
21.540081	1289.747410	15.105267
21.866040	1292.798637	15.110285
21.665646	1290.573580	15.115303
21.568351	1294.432765	15.120320
21.831311	1291.021069	15.125338
21.782938	1292.262642	15.130355
21.887608	1293.215138	15.135373
21.919462	1285.509729	15.140391
21.836652	1280.085082	15.145408
21.886862	1278.253122	15.150426
21.800540	1272.150506	15.155443
21.820572	1279.743692	15.160461
21.926925	1276.258702	15.165479
22.011238	1293.315893	15.170496
22.447595	1279.935879	15.175514
21.947173	1283.507918	15.180531
22.038456	1267.792949	15.185549
22.108006	1266.655418	15.190567
22.059036	1265.454403	15.195584
22.220058	1263.908050	15.200602
22.108115	1268.388085	15.205619
22.184365	1266.690907	15.210637
22.035491	1272.060386	15.215655
21.860430	1271.169471	15.220672
22.182620	1261.644955	15.225690
22.059621	1268.976515	15.230707
21.997752	1267.465085	15.235725
22.281075	1272.545932	15.240743
21.893979	1290.850984	15.245760
22.229279	1292.127120	15.250778
22.388379	1305.552763	15.255795
22.143614	1295.987668	15.260813
22.282883	1295.792300	15.265831
22.169682	1303.428462	15.270848
22.039814	1300.103560	15.275866
21.851571	1288.557162	15.280883
21.986253	1301.601605	15.285901
21.957916	1306.210566	15.290919
21.975814	1324.278620	15.295936
22.206519	1320.537444	15.300954
22.524949	1333.512093	15.305971
22.250102	1330.825307	15.310989
22.647531	1326.183815	15.316007
22.381476	1327.096565	15.321024
22.702530	1317.919350	15.326042
22.454972	1325.494519	15.331059
22.193972	1322.931802	15.336077
22.433525	1315.405284	15.341095
22.273173	1328.537001	15.346112
22.558430	1334.245592	15.351130
22.591983	1344.541319	15.356147
22.760758	1346.108648	15.361165
22.794938	1343.168306	15.366183
22.645353	1342.469064	15.371200
23.045933	1342.226441	15.376218
22.677469	1342.309448	15.381235
22.945950	1347.544127	15.386253
23.095343	1340.584013	15.391271
22.716172	1350.739274	15.396288
23.050226	1350.443955	15.401306
23.046087	1344.962780	15.406323
22.920271	1347.655595	15.411341
23.085768	1350.002954	15.416359
23.152762	1354.833685	15.421376
23.152659	1338.284027	15.426394
23.065503	1341.336872	15.431411
23.239417	1342.471034	15.436429
23.298619	1343.200275	15.441447
22.905039	1345.363820	15.446464
23.117724	1342.569085	15.451482
23.257167	1349.089510	15.456499
23.111292	1345.464138	15.461517
23.205141	1341.952692	15.466535
23.136617	1348.827606	15.471552
22.985933	1341.766179	15.476570
23.440632	1344.563706	15.481587
22.998202	1352.838477	15.486605
23.313244	1345.202285	15.491623
22.663258	1347.235584	15.496640
22.969822	1342.643039	15.501658
22.852110	1349.030180	15.506675
23.193859	1369.723768	15.511693
23.600788	1362.776945	15.516711
23.440105	1375.713081	15.521728
23.743848	1366.494370	15.526746
23.387752	1367.945115	15.531763
23.273592	1370.651887	15.536781
23.706508	1358.168641	15.541799
23.623322	1364.408360	15.546816
23.741233	1370.979506	15.551834
23.765081	1367.946100	15.556851
23.474361	1370.895140	15.561869
23.697021	1359.492606	15.566887
23.283888	1375.296012	15.571904
23.457245	1368.985411	15.576922
23.549182	1370.154510	15.581939
23.156824	1370.730431	15.586957
23.610347	1365.395302	15.591975
23.278295	1375.252848	15.596992
23.487056	1393.360497	15.602010
23.927765	1394.181450	15.607027
23.809785	1388.478246	15.612045
23.669883	1389.169254	15.617063
23.682103	1391.843604	15.622080
23.903093	1392.127757	15.627098
23.991103	1394.089614	15.632115
23.843800	1401.450283	15.637133
24.055533	1392.858228	15.642151
24.062419	1392.503712	15.647168
24.447243	1391.894313	15.652186
24.223236	1386.387611	15.657203
23.962365	1383.562922	15.662221
23.865326	1376.849697	15.667239
23.895975	1380.329077	15.672256
24.324258	1389.098628	15.677274
24.422830	1390.052085	15.682291
24.400470	1391.267498	15.687309
24.346418	1393.807058	15.692327
24.194484	1389.885968	15.697344
24.230916	1382.656346	15.702362
24.351676	1374.327873	15.707379
24.296288	1381.895048	15.712397
24.575284	1383.868007	15.717415
24.490241	1387.829439	15.722432
24.529423	1386.226423	15.727450
24.521025	1380.490273	15.732467
24.173446	1385.875140	15.737485
24.162710	1387.596837	15.742503
24.264169	1401.820568	15.747520
24.449712	1405.379830	15.752538
25.081358	1408.026561	15.757555
24.620123	1409.178189	15.762573
25.029010	1392.971515	15.767591
24.467472	1394.214600	15.772608
24.290879	1385.042737	15.777626
24.968552	1392.147906	15.782643
24.609213	1401.791982	15.787661
25.074343	1397.218762	15.792679
24.941311	1381.384199	15.797696
24.825130	1378.072917	15.802714
25.060987	1375.590140	15.807731
24.632620	1384.408700	15.812749
24.657858	1374.955899	15.817767
24.554704	1387.747323	15.822784
24.704125	1398.709765	15.827802
25.170894	1408.618902	15.832819
24.967023	1412.914551	15.837837
25.179356	1403.552347	15.842855
25.339648	1406.468598	15.847872
24.416120	1388.053243	15.852890
24.953112	1394.688129	15.857907
24.724156	1399.934488	15.862925
25.390596	1398.905407	15.867943
25.323166	1396.959318	15.872960
25.106891	1405.302824	15.877978
25.485391	1405.789527	15.882995
25.356601	1402.016293	15.888013
25.199583	1401.627495	15.893031
25.129186	1394.913245	15.898048
25.251145	1398.526652	15.903066
25.313065	1397.885791	15.908083
25.369700	1402.251079	15.913101
25.415420	1403.408487	15.918119
25.264680	1396.668953	15.923136
25.254577	1402.259735	15.928154
25.757573	1393.218083	15.933171
25.406811	1391.698256	15.938189
25.527486	1392.957532	15.943207
25.501917	1396.310019	15.948224
25.364055	1406.828307	15.953242
25.627525	1394.917562	15.958259
25.321157	1403.262560	15.963277
25.050514	1401.360934	15.968295
25.438575	1394.707401	15.973312
25.359815	1398.087158	15.978330
25.395830	1396.614032	15.983347
25.342269	1405.661066	15.988365
25.391481	1410.961679	15.993383
25.896285	1418.633610	15.998400
25.547714	1424.501503	16.003418
26.033360	1427.048030	16.008435
25.741429	1429.631179	16.013453
26.070516	1415.097017	16.018471
25.750667	1429.860173	16.023488
25.558409	1421.413456	16.028506
26.207974	1418.616534	16.033523
25.986435	1420.797316	16.038541
26.235999	1415.513064	16.043559
26.125333	1417.648070	16.048576
26.116487	1416.229309	16.053594
26.179128	1422.493540	16.058611
25.885562	1430.057026	16.063629
25.854170	1420.445809	16.068647
26.048935	1421.185372	16.073664
26.022652	1424.039336	16.078682
26.246922	1420.980831	16.083699
25.854759	1418.801584	16.088717
26.034670	1416.078248	16.093735
26.221907	1410.472389	16.098752
25.746358	1430.189524	16.103770
25.987435	1424.758269	16.108787
25.913246	1440.180407	16.113805
25.998618	1439.501155	16.118823
26.461120	1443.613505	16.123840
26.419979	1459.279801	16.128858
26.396983	1454.063491	16.133875
26.519452	1453.018647	16.138893
26.572890	1453.720392	16.143911
26.633331	1444.482955	16.148928
26.157657	1460.810654	16.153946
26.577665	1449.973617	16.158963
26.484580	1449.473810	16.163981
26.606203	1454.188707	16.168999
26.401906	1454.839312	16.174016
26.291042	1458.867924	16.179034
26.306166	1444.177793	16.184051
26.454407	1457.715710	16.189069
26.707397	1465.909977	16.194087
26.993384	1467.174917	16.199104
26.827400	1466.740183	16.204122
27.050116	1469.144868	16.209139
26.865230	1454.725919	16.214157
26.822011	1455.073562	16.219175
26.970342	1444.250691	16.224192
26.553421	1448.570262	16.229210
27.212921	1461.649364	16.234227
27.066476	1466.220064	16.239245
26.968487	1471.461703	16.244263
27.115128	1473.862528	16.249280
27.253196	1474.790866	16.254298
26.783607	1457.759209	16.259315
27.041008	1472.968468	16.264333
26.969926	1480.250952	16.269351
27.154595	1468.655476	16.274368
26.966242	1476.578056	16.279386
26.774063	1466.045220	16.284403
26.659823	1471.690212	16.289421
27.003312	1473.296453	16.294439
27.489500	1467.063041	16.299456
26.771310	1476.435163	16.304474
27.159155	1475.143602	16.309491
27.367920	1486.832137	16.314509
27.200552	1497.724348	16.319527
27.292477	1492.714093	16.324544
27.343415	1499.485137	16.329562
27.619536	1491.596193	16.334579
27.421318	1490.143979	16.339597
27.300483	1497.847696	16.344615
27.525551	1498.759248	16.349632
27.679128	1498.631067	16.354650
27.562386	1501.789565	16.359667
27.305234	1496.224903	16.364685
27.566720	1497.061318	16.369703
27.843841	1492.091478	16.374720
27.649638	1495.877523	16.379738
28.094929	1483.916140	16.384755
27.950600	1495.808334	16.389773
27.773168	1499.222505	16.394791
27.934670	1488.593214	16.399808
27.732549	1496.230767	16.404826
28.141637	1493.118044	16.409843
28.312529	1493.457389	16.414861
28.002714	1495.633074	16.419879
27.955931	1480.851623	16.424896
28.159167	1492.900807	16.429914
28.140499	1486.090051	16.434931
27.840818	1494.320429	16.439949
27.811075	1492.324241	16.444967
28.237072	1487.065976	16.449984
28.052071	1501.763879	16.455002
28.328276	1483.649623	16.460019
28.067794	1487.739555	16.465037
27.882322	1496.747341	16.470055
27.950647	1493.142029	16.475072
27.911895	1493.113413	16.480090
28.111645	1504.430969	16.485107
28.150815	1513.766502	16.490125
28.125305	1526.205016	16.495143
28.230671	1519.778777	16.500160
28.390917	1519.154065	16.505178
28.585078	1523.245358	16.510195
28.727325	1521.383174	16.515213
28.320319	1522.557871	16.520231
28.721820	1519.427397	16.525248
28.584508	1523.062516	16.530266
28.712638	1520.116893	16.535283
28.510902	1526.125922	16.540301
28.945457	1521.301829	16.545319
29.056562	1513.457665	16.550336
28.817493	1518.162818	16.555354
28.865635	1517.688221	16.560371
28.833605	1517.911029	16.565389
28.590844	1526.362889	16.570407
28.702380	1512.948385	16.575424
28.202990	1523.624377	16.580442
28.810409	1526.599986	16.585459
29.061555	1512.380929	16.590477
28.866641	1527.430718	16.595495
29.010991	1512.802339	16.600512
28.624789	1521.159900	16.605530
28.743624	1506.200992	16.610547
28.891535	1503.498437	16.615565
28.522437	1525.370297	16.620583
28.823477	1524.783488	16.625600
28.983673	1531.534270	16.630618
29.074090	1533.180169	16.635635
28.958237	1538.623452	16.640653
28.758896	1538.130824	16.645671
28.840685	1537.344826	16.650688
28.994379	1538.911380	16.655706
29.187111	1530.240181	16.660723
29.303661	1524.774756	16.665741
29.012627	1527.048494	16.670759
29.435417	1534.629179	16.675776
29.631782	1553.575264	16.680794
29.686306	1545.045640	16.685811
29.602720	1538.383897	16.690829
29.265415	1530.480590	16.695847
29.360716	1517.863928	16.700864
29.437846	1546.725785	16.705882
29.659640	1547.770403	16.710899
29.933797	1542.314995	16.715917
29.437981	1542.200195	16.720935
29.319064	1534.938044	16.725952
29.578192	1552.908570	16.730970
29.490000	1545.401747	16.735987
29.720571	1547.937762	16.741005
29.856102	1548.595089	16.746023
30.089556	1542.369690	16.751040
29.636058	1552.205333	16.756058
29.771729	1546.377126	16.761075
30.028056	1539.775740	16.766093
29.896429	1546.376580	16.771111
29.784481	1544.222844	16.776128
29.747319	1543.370273	16.781146
30.005260	1550.872647	16.786163
30.063323	1545.750912	16.791181
30.014933	1550.019077	16.796199
30.297214	1550.574512	16.801216
30.196014	1543.830316	16.806234
29.727075	1549.237401	16.811251
30.130860	1543.256728	16.816269
29.639506	1555.187554	16.821287
30.218907	1557.713099	16.826304
30.387881	1563.174882	16.831322
30.276152	1560.582430	16.836339
30.489882	1572.835162	16.841357
30.369641	1579.563626	16.846375
30.713194	1569.284479	16.851392
30.432255	1563.136513	16.856410
30.509890	1566.378182	16.861427
30.418730	1558.815012	16.866445
30.633819	1571.130649	16.871463
30.504446	1564.450823	16.876480
30.676817	1573.819168	16.881498
30.404568	1567.840261	16.886515
30.920651	1568.602073	16.891533
30.630045	1568.732845	16.896551
30.811237	1564.740587	16.901568
30.560643	1563.599546	16.906586
30.591073	1571.371117	16.911603
30.613941	1564.307657	16.916621
31.001699	1560.636503	16.921639
30.968642	1570.191675	16.926656
30.818902	1574.283211	16.931674
31.033038	1576.521988	16.936691
30.968344	1564.176529	16.941709
30.813719	1573.331006	16.946727
30.994345	1567.262206	16.951744
30.919888	1568.877134	16.956762
30.942219	1570.590511	16.961779
31.269456	1564.912174	16.966797
30.647672	1566.770655	16.971815
31.074640	1557.870228	16.976832
30.876158	1563.572631	16.981850
30.692763	1569.490434	16.986867
30.719830	1572.645348	16.991885
30.649499	1589.764923	16.996903
31.015854	1594.873881	17.001920
31.219270	1590.732959	17.006938
31.032933	1591.191396	17.011955
30.960088	1591.938180	17.016973
31.249976	1606.599635	17.021991
31.497702	1613.993177	17.027008
31.633818	1617.336152	17.032026
31.622424	1619.944804	17.037043
31.474167	1613.580361	17.042061
31.421074	1622.545376	17.047079
31.341084	1611.900197	17.052096
31.761376	1616.353735	17.057114
31.504285	1615.365196	17.062131
31.749673	1612.884050	17.067149
31.591695	1619.968755	17.072167
31.648555	1612.117268	17.077184
31.759704	1611.676980	17.082202
31.854908	1620.230574	17.087219
31.876425	1610.090229	17.092237
31.841514	1609.013227	17.097255
32.063842	1610.493290	17.102272
31.943093	1603.468097	17.107290
32.093604	1610.977861	17.112307
32.407401	1609.069852	17.117325
32.228562	1621.494585	17.122343
31.942510	1616.366783	17.127360
32.086728	1612.279315	17.132378
31.693698	1610.526237	17.137395
31.883705	1609.663317	17.142413
32.055908	1606.745489	17.147431
31.916667	1617.873221	17.152448
32.230192	1621.002197	17.157466
32.128151	1636.697126	17.162483
32.738883	1635.638890	17.167501
32.504991	1638.755804	17.172519
32.248744	1633.295105	17.177536
32.531143	1626.986264	17.182554
32.483575	1642.448589	17.187571
32.540025	1640.767102	17.192589
32.299431	1630.323811	17.197607
32.734465	1627.339552	17.202624
32.771352	1634.611493	17.207642
32.536602	1630.883217	17.212659
32.792785	1632.279078	17.217677
32.685983	1628.391892	17.222695
32.719744	1630.570569	17.227712
32.674107	1633.184589	17.232730
32.541814	1632.340606	17.237747
32.935007	1627.866968	17.242765
32.826778	1628.543554	17.247783
32.766160	1631.156764	17.252800
33.203615	1629.112608	17.257818
33.083259	1637.564277	17.262835
33.319062	1629.432267	17.267853
32.827519	1628.243762	17.272871
32.797459	1632.231349	17.277888
33.166544	1623.541942	17.282906
32.824459	1629.465692	17.287923
33.067650	1622.392937	17.292941
32.909063	1621.063898	17.297959
32.668825	1639.652424	17.302976
32.835214	1628.889733	17.307994
32.546042	1637.487779	17.313011
32.826618	1645.740926	17.318029
33.164200	1647.625836	17.323047
33.035607	1664.849291	17.328064
33.180926	1656.207552	17.333082
32.996388	1656.059759	17.338099
33.570144	1654.486578	17.343117
33.524440	1653.594312	17.348135
33.392267	1653.365726	17.353152
33.472210	1663.979435	17.358170
33.518756	1679.966720	17.363187
34.109668	1677.683907	17.368205
33.757809	1671.477583	17.373223
33.814273	1668.486356	17.378240
33.853603	1650.326990	17.383258
33.452215	1657.364635	17.388275
33.710422	1669.055011	17.393293
33.908636	1681.101953	17.398311
34.167046	1676.763036	17.403328
33.979486	1675.810939	17.408346
33.716199	1677.363938	17.413363
33.974299	1673.217586	17.418381
33.967487	1678.432376	17.423399
34.067177	1677.372152	17.428416
34.028838	1685.934077	17.433434
33.975185	1687.028173	17.438451
34.036063	1676.708043	17.443469
34.399139	1689.243587	17.448487
34.132308	1689.323294	17.453504
34.055620	1690.048592	17.458522
33.960782	1678.922833	17.463539
34.149283	1672.518230	17.468557
34.505714	1675.659429	17.473575
34.594153	1675.487801	17.478592
34.453552	1672.211851	17.483610
34.311262	1672.527681	17.488627
34.302189	1675.202253	17.493645
34.295644	1677.314664	17.498663
33.896661	1679.539058	17.503680
34.308210	1688.008404	17.508698
34.520307	1690.910273	17.513715
34.408231	1699.707833	17.518733
34.491272	1697.491967	17.523751
34.463375	1706.140634	17.528768
34.869788	1703.268150	17.533786
34.650926	1697.934125	17.538803
35.144592	1700.965460	17.543821
34.625508	1695.356563	17.548839
34.688860	1699.133857	17.553856
34.619328	1695.177697	17.558874
34.820184	1698.731463	17.563891
34.793725	1698.511562	17.568909
34.485010	1701.678081	17.573927
34.797230	1718.340185	17.578944
35.353120	1726.187294	17.583962
35.413176	1726.070609	17.588979
34.979361	1724.336533	17.593997
35.163419	1716.117911	17.599015
34.779384	1724.825542	17.604032
35.185466	1723.259691	17.609050
35.152230	1728.462856	17.614067
35.159573	1721.202939	17.619085
35.118635	1721.906857	17.624103
34.977645	1728.610223	17.629120
35.086427	1725.632882	17.634138
35.001557	1729.237734	17.639155
35.483374	1744.200610	17.644173
35.659721	1758.681152	17.649191
35.466154	1757.755239	17.654208
35.592466	1756.741336	17.659226
35.272266	1757.836171	17.664243
35.481578	1753.467056	17.669261
36.077562	1754.535115	17.674279
35.569577	1758.181018	17.679296
35.707052	1753.460218	17.684314
35.585262	1752.365260	17.689331
35.654448	1750.252551	17.694349
36.125825	1749.288732	17.699367
35.727509	1751.670830	17.704384
36.222853	1755.418323	17.709402
36.038163	1741.873325	17.714419
36.089326	1746.488879	17.719437
36.212763	1750.155778	17.724455
35.922522	1752.536723	17.729472
36.378447	1747.807058	17.734490
35.979670	1754.320436	17.739507
36.180611	1745.723591	17.744525
36.123970	1739.739248	17.749543
36.043713	1743.535897	17.754560
36.210568	1737.194625	17.759578
36.635752	1743.657801	17.764595
36.185586	1739.095353	17.769613
36.404475	1750.672014	17.774631
36.108925	1768.164739	17.779648
36.361368	1767.421425	17.784666
36.457046	1763.688689	17.789683
36.607970	1762.674086	17.794701
36.826724	1763.394125	17.799719
36.783534	1763.037980	17.804736
36.921106	1757.910039	17.809754
36.908637	1765.877776	17.814771
37.271840	1764.902501	17.819789
36.983429	1752.920187	17.824807
36.997902	1737.178970	17.829824
37.068192	1734.144538	17.834842
36.855294	1732.498931	17.839859
37.165812	1737.165371	17.844877
37.053133	1723.839492	17.849895
36.612977	1728.787657	17.854912
36.797661	1724.457124	17.859930
36.058626	1734.574304	17.864947
37.019952	1752.924190	17.869965
37.672755	1752.932398	17.874983
37.212951	1755.870119	17.880000
36.996834	1753.385518	17.885018
37.061273	1762.909738	17.890035
36.740474	1760.703486	17.895053
37.010385	1753.702237	17.900071
36.662654	1769.618825	17.905088
37.216858	1769.077557	17.910106
37.251070	1775.280089	17.915123
37.390138	1786.850344	17.920141
37.483791	1782.246863	17.925159
37.170716	1789.201291	17.930176
37.705184	1787.899359	17.935194
37.182202	1790.714433	17.940211
37.301321	1785.254838	17.945229
37.883098	1778.580282	17.950247
37.736797	1791.833220	17.955264
37.621280	1785.252133	17.960282
37.822811	1774.837321	17.965299
37.690342	1788.249046	17.970317
37.679541	1782.181763	17.975335
37.970340	1790.546992	17.980352
38.428306	1783.885520	17.985370
38.108859	1785.605128	17.990387
37.985732	1782.686204	17.995405
37.979418	1775.990175	18.000423
37.816046	1781.655585	18.005440
38.020877	1795.030247	18.010458
38.518193	1805.758538	18.015475
38.422557	1805.000328	18.020493
38.331601	1789.102003	18.025511
38.458825	1776.852567	18.030528
38.517436	1771.923198	18.035546
38.451740	1769.493927	18.040563
38.184487	1779.395193	18.045581
38.266763	1785.347186	18.050599
38.452230	1799.570695	18.055616
38.191698	1802.448798	18.060634
38.561217	1801.687140	18.065651
38.659791	1807.358857	18.070669
38.418569	1804.575205	18.075687
38.522777	1811.606282	18.080704
38.665595	1802.624015	18.085722
38.846981	1800.184432	18.090739
38.806812	1808.551029	18.095757
39.024453	1799.945230	18.100775
38.780385	1807.775692	18.105792
38.719893	1812.273048	18.110810
38.709390	1798.975288	18.115827
38.303004	1801.649010	18.120845
38.939046	1824.487288	18.125863
38.870733	1823.440755	18.130880
39.002964	1830.710462	18.135898
39.079422	1830.963617	18.140915
38.946755	1834.711687	18.145933
39.228820	1824.167456	18.150951
38.859595	1826.137880	18.155968
39.324070	1824.869005	18.160986
39.391891	1821.636116	18.166003
39.225921	1829.498535	18.171021
39.407178	1827.532371	18.176039
39.079680	1829.085975	18.181056
39.266019	1831.079815	18.186074
39.217198	1823.579331	18.191091
39.501577	1842.436188	18.196109
39.538297	1852.611781	18.201127
39.808277	1854.469434	18.206144
39.644274	1858.181390	18.211162
39.912449	1847.383684	18.216179
39.709794	1849.858224	18.221197
40.298121	1849.358947	18.226215
39.827927	1836.682331	18.231232
39.773633	1819.152886	18.236250
39.872830	1825.076992	18.241267
39.855146	1840.692606	18.246285
40.251051	1843.452085	18.251303
40.388639	1842.578431	18.256320
39.721056	1828.326334	18.261338
40.115262	1833.197452	18.266355
39.921419	1856.569768	18.271373
39.895170	1844.587346	18.276391
40.261654	1854.395671	18.281408
40.120943	1853.256331	18.286426
40.334596	1847.280099	18.291443
40.478577	1853.096205	18.296461
40.306002	1852.337424	18.301479
40.155154	1856.063099	18.306496
40.006813	1846.855011	18.311514
40.152056	1850.146104	18.316531
40.057893	1847.295220	18.321549
40.291631	1857.007573	18.326567
40.470960	1863.392540	18.331584
40.319466	1869.052961	18.336602
40.507921	1862.963899	18.341619
40.589257	1874.435952	18.346637
40.466480	1870.172493	18.351655
40.386870	1863.468978	18.356672
40.576142	1871.370437	18.361690
40.951953	1879.649800	18.366707
40.715184	1892.137448	18.371725
40.776921	1895.725675	18.376743
41.187698	1895.068010	18.381760
41.113784	1886.173312	18.386778
41.146258	1884.296729	18.391795
41.117111	1892.876248	18.396813
41.195227	1884.251241	18.401831
41.251718	1879.495757	18.406848
40.971104	1888.717475	18.411866
41.306598	1886.462032	18.416883
41.391328	1884.084921	18.421901
41.567938	1883.284053	18.426919
41.361770	1884.433617	18.431936
41.151996	1899.858457	18.436954
41.239697	1882.549717	18.441971
40.798458	1894.782205	18.446989
41.175616	1905.504134	18.452007
41.293998	1903.879195	18.457024
41.524125	1910.328809	18.462042
41.535074	1909.768505	18.467059
41.633151	1918.362819	18.472077
41.859497	1909.048653	18.477095
41.806713	1911.824790	18.482112
41.773321	1912.843137	18.487130
41.891195	1907.525722	18.492147
42.065855	1923.682513	18.497165
42.100327	1922.944941	18.502183
42.059225	1920.764279	18.507200
42.230119	1929.684886	18.512218
42.416356	1919.048308	18.517235
42.063367	1919.567580	18.522253
42.107980	1902.186671	18.527271
42.189281	1909.022545	18.532288
42.007488	1928.621611	18.537306
42.232011	1927.232523	18.542323
42.204367	1934.732463	18.547341
42.329671	1933.816545	18.552359
42.268795	1930.307134	18.557376
42.129556	1938.847116	18.562394
42.566543	1936.282254	18.567411
42.601492	1933.095524	18.572429
42.738309	1931.625496	18.577447
42.417289	1930.056776	18.582464
42.569251	1937.676911	18.587482
42.839893	1925.591110	18.592499
42.801692	1932.161673	18.597517
42.899834	1926.074116	18.602535
42.743755	1922.709020	18.607552
42.836654	1936.953454	18.612570
42.865734	1927.525008	18.617587
43.305224	1934.083849	18.622605
43.131812	1936.490698	18.627623
43.154901	1929.199826	18.632640
43.075757	1932.904814	18.637658
43.438111	1935.148819	18.642675
43.010476	1933.003468	18.647693
43.348207	1941.048968	18.652711
43.332218	1947.496128	18.657728
43.503038	1961.488514	18.662746
43.481963	1953.494442	18.667763
43.626688	1949.053343	18.672781
43.084743	1943.533162	18.677799
43.683504	1951.076986	18.682816
43.654179	1954.875167	18.687834
43.388113	1944.839655	18.692851
43.594244	1955.411673	18.697869
43.968950	1950.076098	18.702887
43.816519	1945.618436	18.707904
43.648542	1949.782348	18.712922
43.891985	1944.372659	18.717939
43.768207	1945.531411	18.722957
43.745185	1945.926395	18.727975
44.130874	1947.087380	18.732992
43.732550	1949.453725	18.738010
43.824097	1943.502905	18.743027
43.927370	1943.420476	18.748045
43.814663	1941.055356	18.753063
44.064085	1945.090748	18.758080
44.012380	1954.270322	18.763098
44.292579	1961.169735	18.768115
44.134846	1970.526887	18.773133
44.077672	1972.880812	18.778151
44.014615	1972.445719	18.783168
43.589259	1973.872646	18.788186
44.123630	1964.882602	18.793203
44.373029	1984.158530	18.798221
44.230589	1995.460579	18.803239
44.582354	1992.991119	18.808256
44.817354	1992.913299	18.813274
45.453001	1971.639842	18.818291
45.423797	1975.838826	18.823309
45.422885	1959.834716	18.828327
45.482179	1952.260430	18.833344
45.270424	1950.450510	18.838362
45.314778	1948.142838	18.843379
45.598614	1939.854829	18.848397
45.382127	1939.588953	18.853415
45.672826	1916.504390	18.858432
45.345328	1915.040835	18.863450
45.304326	1908.590049	18.868467
45.193998	1902.538319	18.873485
45.349431	1914.563718	18.878503
45.650607	1913.755955	18.883520
45.558536	1913.136047	18.888538
45.214743	1912.157918	18.893555
45.214555	1909.689960	18.898573
45.442774	1914.826966	18.903591
45.377526	1915.992325	18.908608
45.376472	1904.340455	18.913626
45.035478	1902.901108	18.918643
45.330017	1918.578333	18.923661
45.331811	1929.052953	18.928679
45.506276	1932.977001	18.933696
45.422547	1942.212083	18.938714
45.360325	1931.974215	18.943731
45.828787	1943.521367	18.948749
45.417154	1948.313633	18.953767
45.925482	1934.489481	18.958784
45.704488	1947.946755	18.963802
45.551152	1963.059827	18.968819
45.949020	1963.199505	18.973837
46.103313	1964.024334	18.978855
46.129031	1960.252022	18.983872
45.888693	1973.229472	18.988890
46.082770	1966.823890	18.993907
45.977061	1965.656966	18.998925
45.904157	1976.783994	19.003943
46.228038	1982.789723	19.008960
46.141103	1990.302132	19.013978
46.279581	1994.506408	19.018995
46.496902	1999.184363	19.024013
46.129680	1996.051166	19.029031
46.570710	1997.831537	19.034048
46.484733	2003.213471	19.039066
46.522705	1999.331925	19.044083
46.712681	2014.612174	19.049101
46.765649	2027.180763	19.054119
47.022505	2026.414656	19.059136
46.723626	2032.126624	19.064154
46.769933	2028.054403	19.069171
47.161358	2022.037636	19.074189
47.049791	2026.378934	19.079207
47.164932	2017.116852	19.084224
47.206820	2031.940599	19.089242
46.909483	2024.510529	19.094259
47.087635	2025.344247	19.099277
47.140053	2028.952897	19.104295
47.125008	2026.449378	19.109312
47.117556	2027.807676	19.114330
47.529713	2031.905960	19.119347
47.075522	2029.136705	19.124365
47.341874	2035.489162	19.129383
47.387879	2042.078134	19.134400
47.390016	2049.298879	19.139418
47.219685	2051.957745	19.144435
47.554230	2049.052284	19.149453
47.364508	2054.109634	19.154471
47.646120	2044.710993	19.159488
47.944303	2049.682429	19.164506
48.239707	2048.228574	19.169523
48.232202	2036.637593	19.174541
48.007104	2045.670798	19.179559
48.549561	2032.731231	19.184576
48.223574	2032.728682	19.189594
48.385107	2031.062255	19.194611
48.171338	2033.058841	19.199629
48.087745	2032.175648	19.204647
48.184340	2018.485375	19.209664
48.704471	2027.086204	19.214682
48.426758	2022.136872	19.219699
48.593913	2020.996626	19.224717
48.319918	2027.231754	19.229735
48.463423	2021.597841	19.234752
48.732992	2030.723961	19.239770
48.533050	2034.387932	19.244787
48.786634	2015.771716	19.249805
48.433049	2024.092838	19.254823
48.717996	2027.504097	19.259840
48.618652	2028.157213	19.264858
48.996684	2031.168850	19.269875
49.119462	2030.177578	19.274893
48.509796	2027.375873	19.279911
49.311864	2040.335227	19.284928
48.911549	2050.513130	19.289946
48.830472	2052.514176	19.294963
48.995162	2056.733297	19.299981
48.910103	2060.063667	19.304999
49.396201	2050.055427	19.310016
49.391766	2048.588585	19.315034
49.150673	2055.149954	19.320051
49.131910	2056.014526	19.325069
49.228798	2059.505753	19.330087
49.169002	2050.406773	19.335104
49.082098	2059.352055	19.340122
49.200719	2072.027163	19.345139
49.710216	2066.799833	19.350157
49.765651	2078.288699	19.355175
49.683356	2077.802964	19.360192
49.915652	2078.435681	19.365210
49.559000	2084.327145	19.370227
49.767970	2087.093859	19.375245
49.609816	2085.941456	19.380263
49.632537	2077.249290	19.385280
49.863421	2074.498933	19.390298
49.850659	2084.764469	19.395315
49.777812	2091.706622	19.400333
49.961722	2100.934569	19.405351
50.167677	2091.326834	19.410368
50.276208	2097.214851	19.415386
50.428512	2111.869873	19.420403
50.544513	2100.035420	19.425421
50.281389	2112.132842	19.430439
50.367794	2101.918931	19.435456
50.356145	2096.688031	19.440474
50.685897	2101.881773	19.445491
50.778008	2095.665705	19.450509
50.872708	2103.960811	19.455527
50.910605	2095.736512	19.460544
50.765386	2090.113098	19.465562
50.510159	2100.542874	19.470579
50.761601	2090.281019	19.475597
50.749193	2099.836394	19.480615
50.969639	2104.696939	19.485632
51.249067	2111.233584	19.490650
51.167503	2117.845726	19.495667
51.057354	2116.562713	19.500685
51.333463	2113.685334	19.505703
51.287048	2112.922554	19.510720
51.457988	2108.284788	19.515738
51.236820	2115.228097	19.520755
51.422464	2106.223189	19.525773
51.466344	2112.358046	19.530791
51.550074	2107.279470	19.535808
51.585244	2112.213231	19.540826
51.349805	2114.311059	19.545843
51.347249	2104.164738	19.550861
51.462575	2112.301970	19.555879
51.425604	2112.127895	19.560896
51.686736	2107.529651	19.565914
51.564759	2113.636842	19.570931
51.513966	2104.937244	19.575949
51.664580	2128.322221	19.580967
51.546472	2132.257437	19.585984
51.962951	2139.930896	19.591002
51.935942	2146.799612	19.596019
52.010153	2148.561725	19.601037
52.096107	2143.530133	19.606055
51.983427	2137.251454	19.611072
52.278502	2134.326915	19.616090
52.095896	2136.485901	19.621107
52.017469	2140.462242	19.626125
51.932541	2159.364671	19.631143
52.136564	2160.260620	19.636160
52.649327	2164.355796	19.641178
52.605964	2170.330758	19.646195
52.925892	2164.359863	19.651213
52.355886	2170.821316	19.656231
52.496136	2174.271054	19.661248
52.667793	2162.850754	19.666266
52.605320	2176.438010	19.671283
52.846491	2180.945004	19.676301
52.776655	2184.004746	19.681319
52.601730	2184.070054	19.686336
52.590171	2186.792434	19.691354
52.868331	2180.032746	19.696371
52.914115	2182.572556	19.701389
52.928564	2193.635535	19.706407
52.949735	2209.873442	19.711424
53.240206	2215.089152	19.716442
53.087729	2216.274509	19.721459
53.233589	2209.576568	19.726477
53.074350	2220.218612	19.731495
53.466493	2214.075426	19.736512
53.665099	2200.766697	19.741530
53.430896	2217.297110	19.746547
53.625908	2226.371890	19.751565
53.911093	2226.324080	19.756583
53.757521	2238.688470	19.761600
54.021222	2230.457136	19.766618
53.918316	2251.069921	19.771635
54.007876	2229.411463	19.776653
54.044140	2237.296028	19.781671
54.106614	2232.782532	19.786688
54.506263	2237.315207	19.791706
54.255660	2237.843694	19.796723
54.660316	2233.645847	19.801741
54.618898	2248.571195	19.806759
54.312193	2241.874715	19.811776
54.697265	2223.338677	19.816794
55.228769	2207.516040	19.821811
55.022012	2180.065316	19.826829
55.028553	2186.395413	19.831847
55.126627	2180.030045	19.836864
55.116019	2172.715949	19.841882
55.428509	2165.149244	19.846899
55.096740	2170.910595	19.851917
55.212689	2170.314895	19.856935
55.076008	2150.178491	19.861952
55.070598	2149.163112	19.866970
55.392500	2143.106701	19.871987
55.138493	2136.742859	19.877005
55.050718	2139.079508	19.882023
54.867052	2144.423136	19.887040
55.063440	2141.331006	19.892058
55.264229	2157.477603	19.897075
55.316700	2166.764051	19.902093
55.581856	2162.048388	19.907111
55.150642	2159.300760	19.912128
55.628758	2166.999291	19.917146
55.540177	2164.311597	19.922163
55.337018	2165.192441	19.927181
55.416663	2166.789589	19.932199
55.419087	2161.237702	19.937216
55.240760	2164.677387	19.942234
54.974806	2168.083462	19.947251
55.604246	2178.766029	19.952269
55.779624	2187.733403	19.957287
55.788382	2194.766962	19.962304
56.078420	2185.019759	19.967322
56.055358	2196.407381	19.972339
55.790298	2193.955635	19.977357
55.800317	2193.973030	19.982375
55.842304	2201.326461	19.987392
56.436477	2217.484067	19.992410
56.378384	2220.598785	19.997427
56.364633	2224.921649	20.002445
56.582712	2218.903572	20.007463
56.066340	2219.312737	20.012480
56.047826	2224.598953	20.017498
56.047760	2230.661834	20.022515
56.222373	2228.103323	20.027533
56.607781	2242.933388	20.032551
56.457759	2246.479117	20.037568
56.565116	2240.383698	20.042586
56.703772	2245.743134	20.047603
56.566479	2256.151366	20.052621
57.065114	2265.623605	20.057639
56.848658	2271.051311	20.062656
57.350415	2272.140480	20.067674
57.092239	2279.888142	20.072691
57.186544	2281.489316	20.077709
57.297236	2281.137455	20.082727
57.366648	2277.304577	20.087744
57.517015	2270.160898	20.092762
57.239697	2275.525551	20.097779
56.995896	2277.640488	20.102797
57.259922	2288.670734	20.107815
57.226842	2296.979639	20.112832
57.578458	2299.777690	20.117850
57.668115	2302.114965	20.122867
57.948354	2298.914987	20.127885
58.236233	2291.137472	20.132903
58.188367	2292.631522	20.137920
58.087154	2282.674142	20.142938
58.258041	2295.489555	20.147955
57.703809	2296.696835	20.152973
58.396867	2291.674232	20.157991
58.132061	2291.703125	20.163008
58.265235	2294.333411	20.168026
58.111617	2293.297059	20.173043
58.521404	2303.468111	20.178061
58.749265	2307.428061	20.183079
58.432395	2315.055535	20.188096
58.787590	2316.050894	20.193114
59.020435	2316.036534	20.198131
58.498804	2317.317609	20.203149
58.746935	2305.777929	20.208167
58.663434	2323.749258	20.213184
58.806776	2312.036626	20.218202
58.844253	2319.207758	20.223219
58.954481	2318.287871	20.228237
59.167047	2309.174492	20.233255
58.608389	2315.375417	20.238272
58.716092	2315.866703	20.243290
59.027780	2306.706234	20.248307
58.878305	2328.633030	20.253325
59.450610	2334.180194	20.258343
58.947085	2336.916554	20.263360
59.452358	2332.055919	20.268378
59.309790	2334.817784	20.273395
59.447776	2346.016150	20.278413
59.498538	2338.603999	20.283431
59.508910	2339.628137	20.288448
59.265806	2340.341661	20.293466
59.706421	2352.429980	20.298483
59.907319	2361.519687	20.303501
59.630165	2365.479872	20.308519
59.518306	2375.312932	20.313536
59.805875	2373.939182	20.318554
60.100634	2371.671126	20.323571
59.856147	2370.655319	20.328589
59.923739	2368.110400	20.333607
60.035853	2385.249490	20.338624
60.118888	2401.903954	20.343642
60.136866	2391.568042	20.348659
60.368230	2393.662199	20.353677
60.464349	2394.635032	20.358695
60.083551	2394.628445	20.363712
60.794129	2399.532210	20.368730
61.092959	2411.813214	20.373747
61.031983	2421.117567	20.378765
60.731645	2401.880768	20.383783
60.733437	2398.020585	20.388800
61.186765	2403.952522	20.393818
61.187214	2408.983331	20.398835
60.939501	2413.775285	20.403853
61.312939	2406.331488	20.408871
61.015435	2410.749352	20.413888
61.193476	2409.048743	20.418906
61.415040	2410.412218	20.423923
61.020145	2406.276481	20.428941
61.397945	2400.170196	20.433959
61.045172	2403.612010	20.438976
61.363822	2407.289488	20.443994
61.500269	2417.288815	20.449011
61.613378	2432.868671	20.454029
62.183166	2435.761963	20.459047
61.805156	2437.449776	20.464064
61.779308	2435.572805	20.469082
62.164665	2430.194391	20.474099
61.808510	2429.909360	20.479117
61.984740	2424.128168	20.484135
62.007831	2428.824044	20.489152
62.036665	2430.167218	20.494170
62.102154	2423.052558	20.499187
62.064238	2426.476606	20.504205
62.133039	2424.512216	20.509223
61.832653	2441.539246	20.514240
62.235680	2449.407470	20.519258
62.443172	2453.661008	20.524275
62.057207	2451.780491	20.529293
62.458146	2447.772545	20.534311
62.356649	2464.490696	20.539328
62.439213	2482.515068	20.544346
62.531622	2478.710105	20.549363
62.529599	2481.408942	20.554381
62.444483	2472.856570	20.559399
62.732967	2489.567297	20.564416
63.095158	2493.067540	20.569434
63.538282	2485.600168	20.574451
64.092622	2474.025029	20.579469
64.251827	2463.341868	20.584487
64.011773	2462.224365	20.589504
64.176040	2460.251326	20.594522
64.327236	2444.611156	20.599539
63.791797	2433.452964	20.604557
64.041601	2422.862940	20.609575
64.030597	2421.905232	20.614592
63.842828	2411.895063	20.619610
63.941211	2414.764370	20.624627
63.879434	2419.890148	20.629645
64.008581	2413.885939	20.634663
63.951603	2420.544839	20.639680
63.919211	2411.422446	20.644698
64.026564	2413.261452	20.649715
63.808225	2412.591875	20.654733
64.497964	2418.104886	20.659751
64.272109	2432.680550	20.664768
64.191784	2441.085295	20.669786
64.636499	2439.431273	20.674803
64.266494	2440.937933	20.679821
64.599175	2438.610273	20.684839
64.434268	2434.672048	20.689856
64.339652	2441.264262	20.694874
64.754469	2429.628952	20.699891
64.390341	2444.639742	20.704909
64.528633	2437.895560	20.709927
64.514319	2457.042884	20.714944
64.462981	2472.541232	20.719962
64.937295	2467.341393	20.724979
64.817497	2469.717820	20.729997
65.010375	2468.529330	20.735015
65.269753	2483.742295	20.740032
65.188213	2482.375870	20.745050
65.555641	2480.976975	20.750067
65.268207	2487.072342	20.755085
65.529175	2483.910069	20.760103
65.127640	2486.829307	20.765120
65.450685	2481.302835	20.770138
65.498851	2480.796648	20.775155
65.150816	2488.233397	20.780173
65.549521	2499.836025	20.785191
65.706490	2507.966912	20.790208
65.606771	2514.919752	20.795226
65.684421	2509.598993	20.800243
66.011392	2524.047086	20.805261
65.956928	2539.375550	20.810279
66.041639	2536.414471	20.815296
65.993220	2534.730394	20.820314
66.526754	2529.035214	20.825331
66.332429	2545.187255	20.830349
66.572883	2535.109925	20.835367
66.261572	2543.793930	20.840384
66.347697	2549.991753	20.845402
66.592412	2556.650777	20.850419
66.612920	2571.648751	20.855437
66.872652	2577.383834	20.860455
67.160857	2574.760136	20.865472
66.729455	2566.773269	20.870490
66.925260	2562.090462	20.875507
66.675214	2570.676509	20.880525
66.954258	2570.534977	20.885543
67.409075	2574.374212	20.890560
67.385599	2587.444373	20.895578
67.706185	2595.619100	20.900595
67.305997	2590.698267	20.905613
67.382732	2588.921986	20.910631
67.336686	2589.339528	20.915648
67.322927	2597.102686	20.920666
67.615659	2587.566307	20.925683
67.390934	2585.963503	20.930701
67.530984	2589.621659	20.935719
67.440796	2594.846622	20.940736
67.529550	2611.626630	20.945754
67.829882	2606.157333	20.950771
67.548919	2621.350920	20.955789
67.831881	2613.589818	20.960807
67.909942	2621.789930	20.965824
67.933313	2635.345145	20.970842
68.330817	2650.647077	20.975859
68.407233	2648.867683	20.980877
68.249931	2651.117450	20.985895
68.359633	2647.192965	20.990912
68.482853	2654.546478	20.995930
68.509342	2647.096974	21.000947
68.744527	2661.903580	21.005965
68.581721	2669.810056	21.010983
68.568606	2670.717958	21.016000
68.327583	2684.156826	21.021018
68.883774	2667.193700	21.026035
68.762876	2670.908538	21.031053
68.874990	2691.484982	21.036071
69.030331	2703.949632	21.041088
69.005584	2701.794718	21.046106
69.473347	2705.010188	21.051123
69.498695	2706.477020	21.056141
69.350834	2698.833879	21.061159
69.669171	2693.317548	21.066176
69.720531	2696.058552	21.071194
70.147699	2701.912627	21.076211
70.022113	2704.299459	21.081229
69.958641	2695.046076	21.086247
70.269820	2694.217777	21.091264
70.005848	2701.963371	21.096282
70.258951	2696.349950	21.101299
70.068517	2708.780405	21.106317
70.770151	2711.952922	21.111335
70.658925	2702.741735	21.116352
70.292411	2701.738715	21.121370
70.511277	2700.599793	21.126387
70.517041	2699.923498	21.131405
70.899972	2700.289614	21.136423
70.915587	2708.379615	21.141440
70.416629	2715.407707	21.146458
70.754130	2718.444750	21.151475
70.744742	2705.692162	21.156493
70.678230	2717.714998	21.161511
71.006065	2716.754686	21.166528
70.863018	2716.603537	21.171546
71.042003	2716.029505	21.176563
70.988261	2727.769448	21.181581
71.195245	2733.272977	21.186599
71.757586	2738.916515	21.191616
71.465439	2741.149546	21.196634
71.462668	2735.711918	21.201651
71.515876	2733.046110	21.206669
71.237525	2739.793466	21.211687
71.469165	2738.153865	21.216704
71.241282	2743.498286	21.221722
71.291669	2754.180394	21.226739
71.632750	2758.836002	21.231757
71.692456	2759.012890	21.236775
71.964291	2756.824127	21.241792
71.580855	2765.042956	21.246810
72.115948	2778.735881	21.251827
72.160337	2785.574716	21.256845
72.098177	2782.687107	21.261863
72.330306	2782.852763	21.266880
72.105487	2780.997461	21.271898
72.403026	2783.267511	21.276915
72.491914	2782.445630	21.281933
72.213821	2790.174537	21.286951
72.709914	2800.105105	21.291968
72.497014	2799.882839	21.296986
72.890809	2804.640666	21.302003
72.921166	2801.871119	21.307021
72.856687	2811.753805	21.312039
73.053870	2800.259666	21.317056
72.990306	2809.810808	21.322074
73.199787	2821.241296	21.327091
73.792885	2827.672247	21.332109
74.047552	2833.922666	21.337127
73.656727	2820.096685	21.342144
73.579102	2810.463562	21.347162
73.705668	2820.764499	21.352179
73.721934	2834.832281	21.357197
73.338343	2836.719844	21.362215
73.872871	2830.361615	21.367232
73.813463	2835.240956	21.372250
73.576361	2832.260813	21.377267
73.531802	2832.485600	21.382285
73.580227	2860.148400	21.387303
73.808099	2857.486770	21.392320
73.649081	2857.808396	21.397338
74.214022	2869.612465	21.402355
74.310093	2882.039181	21.407373
74.260655	2874.039675	21.412391
74.660642	2866.635717	21.417408
74.387248	2876.734230	21.422426
74.367778	2874.512188	21.427443
74.623771	2881.109598	21.432461
74.603851	2887.494586	21.437479
74.808847	2900.406085	21.442496
74.962991	2904.784869	21.447514
75.274930	2904.805460	21.452531
75.183140	2895.247103	21.457549
74.794924	2904.666101	21.462567
75.525725	2898.128755	21.467584
75.183585	2910.220153	21.472602
75.208206	2921.278829	21.477619
75.490719	2916.364567	21.482637
75.553148	2936.999576	21.487655
75.647918	2931.054237	21.492672
75.166707	2923.324356	21.497690
75.733660	2933.038741	21.502707
76.151737	2947.255123	21.507725
76.081311	2955.974177	21.512743
75.978869	2954.232245	21.517760
75.831128	2954.258577	21.522778
76.405830	2945.908755	21.527795
76.630126	2940.773204	21.532813
76.635319	2946.377851	21.537831
76.420964	2940.067478	21.542848
76.295153	2947.176070	21.547866
76.560007	2941.623856	21.552883
76.544553	2956.627785	21.557901
76.804144	2964.382992	21.562919
76.934341	2979.199996	21.567936
76.987423	2982.354238	21.572954
76.756255	2972.852396	21.577971
76.963526	2979.719441	21.582989
76.909805	2975.148215	21.588007
77.471760	2965.970296	21.593024
77.328995	2978.731182	21.598042
77.408953	2974.798662	21.603059
77.487528	2970.847421	21.608077
77.432621	2989.196835	21.613095
77.455698	2991.999127	21.618112
77.424994	3005.181190	21.623130
77.713592	3008.225945	21.628147
77.699581	3006.429121	21.633165
77.612333	3004.053559	21.638183
77.760454	3004.642688	21.643200
77.504985	3009.918916	21.648218
77.413378	3017.116862	21.653235
77.997545	3019.815469	21.658253
77.860840	3030.088337	21.663271
78.126745	3041.058784	21.668288
78.342732	3046.980777	21.673306
78.156521	3052.018917	21.678323
78.251748	3049.870414	21.683341
78.148918	3049.116434	21.688359
78.514369	3069.060246	21.693376
78.825455	3079.790076	21.698394
78.843873	3083.988169	21.703411
79.064790	3078.338642	21.708429
78.812506	3083.021020	21.713447
79.184615	3069.315189	21.718464
78.865612	3081.784981	21.723482
79.017246	3089.263626	21.728499
79.431673	3098.806312	21.733517
79.446345	3104.718834	21.738535
79.728497	3101.609948	21.743552
79.579890	3096.939933	21.748570
79.477731	3096.555125	21.753587
80.111854	3100.177007	21.758605
80.027617	3104.618438	21.763623
80.200811	3087.175208	21.768640
79.823166	3101.118695	21.773658
80.126041	3118.856687	21.778675
80.127620	3108.784902	21.783693
80.243146	3128.117751	21.788711
80.449700	3121.870775	21.793728
80.464645	3128.092574	21.798746
80.092577	3121.892066	21.803763
80.184748	3118.364756	21.808781
80.493629	3135.865105	21.813799
80.776152	3139.081271	21.818816
80.938183	3133.261047	21.823834
81.101493	3134.516925	21.828851
81.507382	3134.387079	21.833869
81.495827	3133.246358	21.838887
81.466415	3128.431409	21.843904
81.685262	3132.705423	21.848922
81.426567	3133.506638	21.853939
81.769850	3130.798481	21.858957
81.846595	3127.942710	21.863975
81.701035	3125.951860	21.868992
81.657863	3127.249556	21.874010
81.993960	3121.790282	21.879027
82.109747	3130.754839	21.884045
81.677923	3126.113408	21.889063
81.983179	3133.100879	21.894080
81.765589	3133.889341	21.899098
82.027823	3125.455831	21.904115
82.009280	3126.090013	21.909133
81.630663	3141.756993	21.914151
82.145974	3152.259182	21.919168
82.326222	3149.393503	21.924186
82.201338	3157.423656	21.929203
82.470564	3161.980159	21.934221
82.660162	3182.586055	21.939239
82.456874	3192.657979	21.944256
82.610191	3187.785979	21.949274
82.433662	3180.516407	21.954291
82.626360	3184.005467	21.959309
82.738428	3205.762945	21.964327
82.695961	3214.641868	21.969344
82.838339	3210.027234	21.974362
83.049412	3221.934321	21.979379
83.172983	3233.530031	21.984397
82.970574	3244.839100	21.989415
83.445045	3238.988829	21.994432
83.359869	3238.241543	21.999450
83.211648	3247.137052	22.004467
83.739212	3253.262798	22.009485
83.674071	3256.113672	22.014503
84.006793	3263.617674	22.019520
83.951868	3259.737787	22.024538
83.921688	3269.088252	22.029555
84.102731	3279.406167	22.034573
84.238566	3282.743186	22.039591
84.432224	3285.600861	22.044608
84.618035	3283.387638	22.049626
84.693492	3283.325344	22.054643
84.951450	3272.749328	22.059661
84.953344	3273.178312	22.064679
85.252901	3269.097696	22.069696
85.345700	3270.099504	22.074714
85.110008	3269.195892	22.079731
84.909982	3271.240959	22.084749
84.863432	3271.589157	22.089767
85.043004	3283.567503	22.094784
85.394983	3282.316158	22.099802
85.000084	3302.492983	22.104819
85.317034	3296.162368	22.109837
85.706291	3296.350756	22.114855
85.497505	3304.782341	22.119872
85.981853	3303.166223	22.124890
86.296400	3311.064471	22.129907
86.343074	3313.768428	22.134925
86.250310	3313.637801	22.139943
86.656920	3313.375279	22.144960
86.808052	3307.528301	22.149978
86.910621	3299.479540	22.154995
86.736339	3279.360390	22.160013
87.063559	3271.547884	22.165031
86.837217	3274.632331	22.170048
87.307668	3271.487602	22.175066
86.844377	3277.096313	22.180083
87.072182	3278.237939	22.185101
87.260610	3272.937475	22.190119
87.029394	3269.927930	22.195136
87.257758	3268.882174	22.200154
87.101839	3276.039799	22.205171
87.131314	3272.257155	22.210189
87.240312	3287.529081	22.215207
87.325283	3294.128187	22.220224
87.370236	3300.487376	22.225242
87.292107	3302.983634	22.230259
87.223044	3299.547831	22.235277
87.445936	3321.007176	22.240295
87.872853	3327.656878	22.245312
87.586486	3316.781051	22.250330
87.539881	3328.368765	22.255347
87.532179	3334.505808	22.260365
87.830600	3354.110091	22.265383
87.801959	3356.529164	22.270400
88.208786	3365.041078	22.275418
88.192643	3377.356309	22.280435
88.385261	3384.655060	22.285453
88.771985	3383.070012	22.290471
88.442504	3385.425752	22.295488
88.506722	3378.301446	22.300506
88.419308	3392.944569	22.305523
88.836096	3404.229320	22.310541
89.093051	3415.576996	22.315559
88.892508	3409.444203	22.320576
88.768534	3409.438405	22.325594
88.625830	3414.782302	22.330611
88.942026	3431.808349	22.335629
89.302262	3445.311395	22.340647
89.185818	3439.449482	22.345664
89.524339	3449.717572	22.350682
89.287101	3470.305450	22.355699
90.010626	3467.727049	22.360717
89.824743	3465.237470	22.365735
89.982602	3471.414902	22.370752
90.312976	3464.371959	22.375770
90.088202	3476.511628	22.380787
90.380312	3482.418682	22.385805
90.838719	3492.033595	22.390823
90.482787	3495.050005	22.395840
90.596161	3490.228371	22.400858
90.709652	3491.166980	22.405875
90.642220	3482.541919	22.410893
90.626852	3482.815797	22.415911
90.958695	3485.680261	22.420928
90.948123	3493.061392	22.425946
91.117168	3504.697496	22.430963
91.208110	3508.991639	22.435981
91.372363	3502.170399	22.440999
91.229419	3504.351739	22.446016
91.417651	3509.940508	22.451034
91.314481	3518.415615	22.456051
91.430929	3529.068893	22.461069
91.538697	3535.888614	22.466087
91.884943	3536.279436	22.471104
92.068489	3527.479310	22.476122
92.116415	3528.324034	22.481139
91.950585	3528.324794	22.486157
92.027294	3537.109452	22.491175
92.381072	3547.700308	22.496192
92.919514	3544.323938	22.501210
92.815318	3555.491561	22.506227
92.481418	3561.531440	22.511245
92.845625	3560.256068	22.516263
92.797886	3553.559555	22.521280
92.964591	3556.178460	22.526298
92.934206	3558.872433	22.531315
93.320489	3567.179345	22.536333
93.506139	3574.510828	22.541351
93.301829	3579.539325	22.546368
93.726372	3578.548036	22.551386
93.544102	3575.246702	22.556403
93.845131	3575.313195	22.561421
93.863977	3576.089882	22.566439
93.794483	3579.291840	22.571456
93.816728	3574.771687	22.576474
93.653377	3584.152648	22.581491
93.560061	3576.557403	22.586509
93.895507	3594.274978	22.591527
93.646847	3603.445217	22.596544
94.011582	3607.967932	22.601562
93.995796	3614.002176	22.606579
94.040441	3623.123315	22.611597
94.561103	3626.415887	22.616615
94.215078	3628.228205	22.621632
94.453934	3628.051933	22.626650
94.562040	3632.914712	22.631667
94.721383	3648.977607	22.636685
94.951382	3651.529796	22.641703
94.838128	3651.699073	22.646720
95.034403	3643.348252	22.651738
95.173550	3663.839505	22.656755
95.258801	3668.601716	22.661773
95.814455	3668.066489	22.666791
96.112791	3663.891286	22.671808
95.897768	3670.218741	22.676826
96.103723	3670.126531	22.681843
95.959668	3674.309184	22.686861
96.421142	3660.049173	22.691879
96.177842	3671.765770	22.696896
96.432657	3654.233455	22.701914
96.643135	3670.572428	22.706931
96.280339	3666.099951	22.711949
96.717273	3656.395228	22.716967
96.654848	3658.301995	22.721984
96.748412	3663.994021	22.727002
96.217207	3664.093057	22.732019
96.368197	3675.242867	22.737037
96.709158	3682.155519	22.742055
96.571703	3688.764367	22.747072
97.037284	3689.414254	22.752090
97.361517	3702.168767	22.757107
97.117902	3711.300393	22.762125
97.485478	3707.587785	22.767143
97.101416	3722.523845	22.772160
97.316448	3719.267554	22.777178
97.949454	3727.166592	22.782195
97.876172	3749.073704	22.787213
98.259996	3735.987337	22.792231
98.201556	3741.056151	22.797248
98.182043	3736.346806	22.802266
98.362849	3744.812247	22.807283
98.496467	3746.394768	22.812301
98.188268	3743.185728	22.817319
97.986601	3733.928213	22.822336
98.172326	3756.318709	22.827354
98.617440	3764.300859	22.832371
98.401282	3769.037723	22.837389
98.627920	3769.974402	22.842407
98.739862	3785.151595	22.847424
99.023743	3796.624703	22.852442
98.797381	3792.654776	22.857459
98.994935	3798.453650	22.862477
99.250502	3804.470696	22.867495
99.238863	3822.119776	22.872512
99.578380	3820.368487	22.877530
99.371453	3817.989473	22.882547
99.449615	3831.366557	22.887565
100.164451	3828.688465	22.892583
100.403137	3848.776099	22.897600
100.519912	3846.797727	22.902618
100.436892	3841.296586	22.907635
100.298671	3841.081542	22.912653
100.761299	3842.732467	22.917671
100.981534	3840.851515	22.922688
100.742059	3833.559978	22.927706
100.918461	3832.213007	22.932723
100.783602	3844.114733	22.937741
100.834858	3830.382845	22.942759
100.612387	3842.389830	22.947776
100.927605	3849.423365	22.952794
101.215571	3859.153557	22.957811
100.905873	3875.204916	22.962829
101.096277	3870.260640	22.967847
100.803841	3871.913079	22.972864
101.057524	3876.137624	22.977882
101.544669	3885.274789	22.982899
101.413729	3901.967318	22.987917
101.517572	3892.885959	22.992935
101.563542	3908.565987	22.997952
101.202880	3925.496537	23.002970
101.597679	3913.595123	23.007987
101.603309	3941.020083	23.013005
102.158299	3943.562430	23.018023
101.956724	3947.384859	23.023040
102.400579	3966.679791	23.028058
102.701860	3976.546841	23.033075
102.312332	3973.921809	23.038093
102.568893	3979.458985	23.043111
102.720286	3993.667473	23.048128
102.910722	4002.791213	23.053146
103.206805	4003.145716	23.058163
103.235486	3996.885274	23.063181
103.409735	4000.064901	23.068199
103.423620	4005.842116	23.073216
103.321266	4013.102112	23.078234
103.665174	4016.927474	23.083251
103.960055	4026.966000	23.088269
104.646225	4024.920495	23.093287
104.080448	4026.899849	23.098304
104.224380	4020.921200	23.103322
104.482809	4019.087905	23.108339
104.135271	4017.254857	23.113357
104.438206	4028.100160	23.118375
104.883910	4044.992864	23.123392
104.765631	4043.853024	23.128410
104.972033	4046.096482	23.133427
104.610009	4052.680674	23.138445
104.488677	4047.157066	23.143463
104.876583	4045.628592	23.148480
105.062447	4069.038971	23.153498
105.072263	4061.118036	23.158515
105.214476	4070.568162	23.163533
105.431121	4069.884028	23.168551
105.483231	4082.062788	23.173568
105.419794	4090.484591	23.178586
105.827212	4091.254081	23.183603
105.757348	4098.613183	23.188621
105.633100	4090.141929	23.193639
106.000969	4105.569684	23.198656
106.151051	4114.055894	23.203674
106.492377	4115.990988	23.208691
106.390204	4118.390119	23.213709
106.875852	4121.770336	23.218727
106.503672	4129.820725	23.223744
106.527781	4136.344450	23.228762
106.996661	4141.150844	23.233779
106.902342	4151.603935	23.238797
106.961415	4150.499430	23.243815
107.196000	4143.054585	23.248832
107.118359	4162.541904	23.253850
107.632503	4169.307666	23.258867
107.346819	4165.356419	23.263885
107.411070	4175.948815	23.268903
107.631970	4184.098850	23.273920
107.317982	4189.441402	23.278938
107.994488	4197.756795	23.283955
108.213194	4206.229140	23.288973
108.221783	4194.340705	23.293991
108.264662	4195.224129	23.299008
108.291870	4200.689988	23.304026
108.267854	4201.558641	23.309043
108.511571	4221.667996	23.314061
109.109469	4226.640429	23.319079
109.025607	4224.955434	23.324096
109.237907	4223.334515	23.329114
109.003209	4215.672771	23.334131
108.801173	4221.259776	23.339149
109.118657	4224.432784	23.344167
109.296081	4218.915976	23.349184
109.349459	4228.133900	23.354202
109.878543	4239.928707	23.359219
109.505702	4246.290556	23.364237
109.683704	4243.046286	23.369255
109.720960	4238.905544	23.374272
109.720904	4241.951544	23.379290
110.278408	4265.846859	23.384307
109.986435	4272.110823	23.389325
109.802576	4270.027997	23.394343
109.719858	4267.768346	23.399360
110.027168	4284.654550	23.404378
110.289737	4287.615221	23.409395
110.410774	4301.961277	23.414413
110.524914	4314.471371	23.419431
110.805982	4317.902617	23.424448
110.911454	4328.908451	23.429466
110.953206	4324.770142	23.434483
110.827740	4344.205176	23.439501
111.104089	4354.934895	23.444519
111.344642	4338.774058	23.449536
111.349254	4359.246141	23.454554
111.856823	4365.268082	23.459571
111.820327	4371.185878	23.464589
111.739417	4376.867587	23.469607
112.061949	4375.519778	23.474624
112.211474	4388.983944	23.479642
112.445320	4388.167689	23.484659
112.850125	4399.331840	23.489677
112.287905	4384.941252	23.494695
112.881324	4389.046404	23.499712
112.484472	4386.469805	23.504730
113.173877	4394.713827	23.509747
113.576956	4392.848363	23.514765
113.818922	4388.211515	23.519783
114.004634	4381.115128	23.524800
113.839329	4376.816702	23.529818
114.010479	4365.016319	23.534835
114.251364	4369.823774	23.539853
114.181742	4371.340342	23.544871
114.214839	4361.818459	23.549888
114.094909	4354.119737	23.554906
114.436095	4352.510179	23.559923
114.378894	4361.726557	23.564941
114.412752	4356.036500	23.569959
114.777989	4364.987839	23.574976
114.548364	4388.915099	23.579994
114.611071	4386.329630	23.585011
114.928999	4389.916094	23.590029
114.635275	4387.680017	23.595047
115.179311	4376.663982	23.600064
114.947756	4378.332179	23.605082
115.162926	4380.833136	23.610099
115.201085	4406.148343	23.615117
115.141142	4402.221649	23.620135
115.269589	4405.822021	23.625152
115.254095	4412.339425	23.630170
115.341912	4434.039048	23.635187
115.411797	4440.647249	23.640205
114.994835	4441.028251	23.645223
115.649477	4461.439643	23.650240
115.576804	4475.052317	23.655258
115.436782	4474.777574	23.660275
116.019649	4492.514083	23.665293
115.565464	4507.603814	23.670311
116.201861	4514.195885	23.675328
116.024310	4527.960759	23.680346
116.673223	4530.292774	23.685363
116.863070	4546.616831	23.690381
116.640574	4557.996150	23.695399
116.612661	4558.736014	23.700416
116.969515	4570.545395	23.705434
117.479895	4585.534575	23.710451
117.470141	4592.347855	23.715469
117.390624	4585.390794	23.720487
117.719738	4597.873716	23.725504
117.784302	4609.346978	23.730522
118.021840	4611.863402	23.735539
118.317704	4607.135985	23.740557
118.125522	4604.770338	23.745575
118.518857	4601.003011	23.750592
118.417725	4624.645304	23.755610
118.593290	4616.868610	23.760627
118.683047	4623.988275	23.765645
118.941437	4632.334655	23.770663
119.006977	4627.725387	23.775680
119.317461	4640.220727	23.780698
119.312984	4650.609524	23.785715
119.503157	4651.728728	23.790733
119.782357	4650.359280	23.795751
119.635139	4646.701885	23.800768
119.918264	4652.897974	23.805786
119.903100	4647.408053	23.810803
120.368488	4647.272039	23.815821
120.269717	4658.480523	23.820839
120.682686	4661.057851	23.825856
120.492098	4662.564986	23.830874
121.026465	4662.358192	23.835891
121.070965	4661.934589	23.840909
120.866361	4659.356238	23.845927
121.495138	4662.382702	23.850944
121.140848	4660.074011	23.855962
121.326641	4647.904996	23.860979
121.370046	4656.736450	23.865997
121.467099	4645.196859	23.871015
121.372069	4649.993886	23.876032
121.015544	4658.364017	23.881050
121.120655	4672.031055	23.886067
121.366803	4677.677400	23.891085
121.595615	4692.518235	23.896103
121.830746	4697.077314	23.901120
121.775732	4702.344719	23.906138
121.714011	4707.108134	23.911155
121.877119	4725.109496	23.916173
121.751550	4736.814644	23.921191
121.971272	4747.998538	23.926208
122.333968	4769.769132	23.931226
122.890236	4770.518490	23.936243
122.712545	4778.128343	23.941261
122.838730	4789.686762	23.946279
123.197628	4785.441843	23.951296
123.207803	4795.219217	23.956314
123.634885	4807.478604	23.961331
124.034964	4806.304851	23.966349
123.590237	4821.068235	23.971367
124.136179	4815.070536	23.976384
123.983815	4825.981336	23.981402
123.968796	4813.562740	23.986419
124.005947	4812.635239	23.991437
123.978508	4828.482232	23.996455
124.480580	4836.146595	24.001472
124.333437	4846.248515	24.006490
124.585987	4844.450782	24.011507
124.626934	4855.416540	24.016525
124.765796	4863.248297	24.021543
124.949991	4875.050205	24.026560
125.001107	4875.099044	24.031578
125.547431	4877.980635	24.036595
125.680255	4879.048863	24.041613
125.423837	4896.159687	24.046631
125.700958	4889.329714	24.051648
125.756255	4893.863356	24.056666
125.968814	4902.895700	24.061683
125.838331	4893.377072	24.066701
125.739581	4915.245387	24.071719
126.028443	4913.625039	24.076736
125.775348	4927.301040	24.081754
126.451445	4954.764532	24.086771
126.586493	4949.885455	24.091789
126.651996	4957.346802	24.096807
126.780161	4960.881040	24.101824
126.943373	4970.760795	24.106842
127.300880	4984.088651	24.111859
127.534406	4981.593127	24.116877
127.371253	4985.813794	24.121895
127.557490	4985.828837	24.126912
127.155463	4998.679108	24.131930
127.626970	5004.968910	24.136947
127.778053	5006.349943	24.141965
127.534945	5025.311709	24.146983
127.914833	5027.708035	24.152000
128.219597	5039.254417	24.157018
128.416236	5052.938967	24.162035
128.663049	5055.561323	24.167053
128.093129	5075.533943	24.172071
128.705429	5071.520724	24.177088
129.047210	5083.976744	24.182106
129.006416	5085.207918	24.187123
129.271448	5082.012997	24.192141
129.152847	5090.478626	24.197159
129.470071	5093.380363	24.202176
129.994178	5109.674653	24.207194
129.992898	5115.170503	24.212211
130.230121	5109.997596	24.217229
130.363815	5114.042365	24.222247
130.372764	5104.432337	24.227264
130.567546	5119.266226	24.232282
130.052359	5136.389406	24.237299
130.612266	5130.332598	24.242317
130.638478	5130.732564	24.247335
131.010674	5130.967844	24.252352
131.345995	5136.650867	24.257370
131.460896	5147.235893	24.262387
131.574080	5146.268054	24.267405
131.790696	5151.268915	24.272423
131.760403	5152.479509	24.277440
131.825983	5156.149854	24.282458
131.748002	5149.747897	24.287475
131.930260	5147.238288	24.292493
131.564229	5148.460446	24.297511
132.339992	5170.195214	24.302528
132.481041	5178.588639	24.307546
132.269193	5185.979894	24.312563
132.744954	5178.648360	24.317581
132.604357	5185.280338	24.322599
132.916404	5188.056637	24.327616
132.764387	5198.901317	24.332634
132.848054	5192.947510	24.337651
132.691864	5193.297139	24.342669
132.618836	5203.324512	24.347687
133.122980	5220.164965	24.352704
133.162573	5219.069761	24.357722
133.339972	5232.274499	24.362739
133.447622	5254.581219	24.367757
133.379228	5260.267555	24.372775
133.411716	5270.382602	24.377792
133.818684	5276.240684	24.382810
133.685708	5292.252975	24.387827
134.132406	5301.728641	24.392845
134.285984	5316.543893	24.397863
134.271624	5316.508292	24.402880
134.852526	5340.859068	24.407898
134.667374	5341.102755	24.412915
134.952794	5344.037925	24.417933
135.026692	5363.834233	24.422951
135.167625	5367.540165	24.427968
135.592746	5366.646552	24.432986
135.562864	5387.163074	24.438003
135.874367	5391.252650	24.443021
135.641633	5391.159719	24.448039
135.862657	5404.910159	24.453056
136.123724	5406.450763	24.458074
136.256987	5421.644923	24.463091
136.674405	5418.391347	24.468109
136.283419	5424.753288	24.473127
136.562825	5444.217605	24.478144
136.726730	5443.522746	24.483162
136.832830	5455.870739	24.488179
136.841869	5464.281821	24.493197
137.278664	5475.593143	24.498215
137.295720	5479.959306	24.503232
137.380764	5482.818564	24.508250
137.213473	5509.000846	24.513267
137.670993	5515.049955	24.518285
137.546251	5529.151386	24.523303
137.574029	5526.419707	24.528320
138.072518	5534.255388	24.533338
138.342752	5555.154385	24.538355
138.321420	5561.995094	24.543373
138.420183	5570.606821	24.548391
138.744450	5577.870048	24.553408
138.799313	5583.063673	24.558426
139.174932	5596.183956	24.563443
139.307580	5600.194275	24.568461
139.330603	5608.899959	24.573479
139.442858	5612.582024	24.578496
139.976196	5617.536550	24.583514
140.001071	5626.393473	24.588531
140.127364	5621.487179	24.593549
140.425221	5634.038844	24.598567
140.272031	5630.088615	24.603584
140.815325	5628.624058	24.608602
140.460536	5637.947680	24.613619
140.680914	5642.723962	24.618637
140.676480	5644.249362	24.623655
141.253270	5646.886399	24.628672
141.312156	5639.752574	24.633690
141.605255	5646.408316	24.638707
141.963863	5669.579036	24.643725
142.218301	5671.120702	24.648743
141.853032	5679.985110	24.653760
142.110011	5672.375145	24.658778
142.311815	5679.398751	24.663795
142.583839	5664.825939	24.668813
142.326287	5666.173185	24.673831
142.462532	5670.059844	24.678848
142.659745	5664.425860	24.683866
142.704985	5664.885991	24.688883
142.741685	5670.865344	24.693901
142.904010	5681.904127	24.698919
143.040319	5686.305319	24.703936
143.080608	5694.525367	24.708954
142.942267	5704.768432	24.713971
143.410166	5708.931436	24.718989
143.206483	5720.097031	24.724007
143.198228	5721.768244	24.729024
143.558419	5738.139285	24.734042
143.729600	5740.461078	24.739059
144.062155	5759.645929	24.744077
144.346908	5778.932991	24.749095
144.205764	5771.439022	24.754112
144.466799	5775.208295	24.759130
144.376965	5800.425534	24.764147
144.360507	5800.087217	24.769165
144.533724	5812.472286	24.774183
144.792527	5830.128292	24.779200
145.363583	5834.193089	24.784218
145.351708	5848.886328	24.789235
145.649667	5849.474176	24.794253
145.941418	5854.555005	24.799271
145.957920	5862.387421	24.804288
145.925742	5870.148549	24.809306
146.029714	5880.341123	24.814323
146.008726	5878.785020	24.819341
146.621392	5888.717969	24.824359
146.678880	5912.649593	24.829376
146.752031	5904.613763	24.834394
146.838125	5907.523432	24.839411
147.119821	5930.791765	24.844429
147.219600	5933.311016	24.849447
147.423891	5940.084951	24.854464
147.664831	5941.439351	24.859482
147.878514	5964.547919	24.864499
148.294232	5954.037182	24.869517
148.405748	5960.494202	24.874535
148.180339	5968.418228	24.879552
148.291192	5966.137509	24.884570
148.132243	5977.116318	24.889587
148.451285	5991.650499	24.894605
148.552799	5991.129545	24.899623
148.649404	6013.704088	24.904640
148.849927	6012.384749	24.909658
148.652250	6021.589248	24.914675
148.988941	6034.018305	24.919693
149.299903	6042.016168	24.924711
149.028493	6046.651789	24.929728
149.563216	6058.525817	24.934746
149.582348	6068.807549	24.939763
150.055852	6087.916999	24.944781
149.946643	6090.207002	24.949799
149.807129	6096.362468	24.954816
150.297097	6121.732384	24.959834
150.442142	6127.729637	24.964851
150.489361	6131.731358	24.969869
150.472072	6150.614715	24.974887
150.715799	6154.112140	24.979904
151.097262	6167.156157	24.984922
151.397141	6174.413973	24.989939
151.616292	6190.236141	24.994957
151.887053	6195.986433	24.999975
152.074663	6215.147119	25.004992
152.059585	6201.127102	25.010010
152.014332	6209.553346	25.015027
152.269191	6205.352813	25.020045
152.836280	6211.615435	25.025063
152.641432	6230.144721	25.030080
153.150246	6229.402111	25.035098
153.239509	6230.047923	25.040115
153.110791	6219.316122	25.045133
153.366549	6222.956887	25.050151
153.470274	6240.934323	25.055168
154.019258	6242.726630	25.060186
153.803461	6251.757303	25.065203
154.089594	6246.472241	25.070221
154.448057	6252.638134	25.075239
154.274606	6251.282664	25.080256
154.089901	6269.437900	25.085274
154.317642	6277.935050	25.090291
154.171011	6274.548718	25.095309
154.696345	6281.032568	25.100327
154.430550	6303.973609	25.105344
155.133700	6307.089722	25.110362
155.351155	6327.382296	25.115379
155.036519	6334.079836	25.120397
155.501906	6327.478694	25.125415
155.532176	6342.254116	25.130432
155.838641	6353.485385	25.135450
156.179573	6357.242262	25.140467
156.077100	6356.977390	25.145485
156.369976	6373.545799	25.150503
156.418666	6378.677480	25.155520
156.441612	6378.976968	25.160538
156.679393	6401.447793	25.165555
156.938256	6404.027420	25.170573
157.183422	6405.949420	25.175591
157.099880	6425.853619	25.180608
157.326062	6434.692022	25.185626
157.312762	6451.807246	25.190643
157.572979	6453.606934	25.195661
158.132533	6459.981311	25.200679
157.866110	6473.461671	25.205696
158.005142	6458.946948	25.210714
158.272977	6487.701559	25.215731
158.141085	6493.161462	25.220749
158.553459	6498.163594	25.225767
158.700555	6517.204670	25.230784
158.695574	6514.039178	25.235802
158.821284	6533.879143	25.240819
158.898973	6538.832700	25.245837
159.521613	6550.743785	25.250855
159.590396	6572.654126	25.255872
159.912747	6564.762063	25.260890
160.339116	6565.980127	25.265907
160.166126	6595.814159	25.270925
160.164701	6591.319065	25.275943
160.754629	6597.780281	25.280960
160.837179	6600.507518	25.285978
161.121383	6604.456431	25.290995
160.943050	6614.993542	25.296013
160.987717	6616.394527	25.301031
161.203929	6629.123823	25.306048
161.560561	6643.902025	25.311066
161.529162	6644.532029	25.316083
161.334225	6659.153577	25.321101
161.915761	6668.271049	25.326119
161.817154	6690.674968	25.331136
162.143783	6688.369827	25.336154
162.239701	6703.766627	25.341171
162.359060	6711.043468	25.346189
163.046000	6719.655138	25.351207
162.831059	6721.813411	25.356224
163.016791	6731.046590	25.361242
162.848579	6748.966106	25.366259
162.642369	6751.009368	25.371277
162.997603	6761.093616	25.376295
163.258007	6777.099240	25.381312
163.191964	6782.343715	25.386330
163.812503	6797.841503	25.391347
163.789373	6804.635604	25.396365
164.301340	6816.276926	25.401383
164.493755	6816.000572	25.406400
164.438639	6836.011253	25.411418
164.800844	6838.798891	25.416435
164.816845	6846.350842	25.421453
165.261391	6856.638977	25.426471
165.220693	6860.020096	25.431488
165.087565	6878.436187	25.436506
165.754584	6874.227757	25.441523
165.740192	6882.390609	25.446541
165.958134	6890.384476	25.451559
166.589572	6892.239698	25.456576
166.539922	6892.323271	25.461594
166.741424	6890.580694	25.466611
167.094478	6893.906446	25.471629
167.649659	6905.013853	25.476647
167.274767	6916.323800	25.481664
167.176689	6909.611842	25.486682
167.453171	6902.680205	25.491699
167.747062	6909.973978	25.496717
168.171754	6919.507603	25.501735
167.943544	6928.919380	25.506752
167.843017	6932.458260	25.511770
168.413871	6928.072313	25.516787
167.937915	6936.989390	25.521805
168.504591	6944.170989	25.526823
168.646659	6960.005898	25.531840
168.742750	6978.490357	25.536858
168.947890	6984.254335	25.541875
169.059418	6993.281444	25.546893
169.216954	7000.239884	25.551911
169.547720	7013.882791	25.556928
169.396469	7019.071231	25.561946
170.142718	7032.898457	25.566963
169.715548	7051.528104	25.571981
170.043551	7046.286766	25.576999
170.478965	7057.943392	25.582016
170.480376	7081.399158	25.587034
170.441524	7082.156622	25.592051
171.034584	7094.195817	25.597069
171.091271	7097.902672	25.602087
171.320920	7106.908174	25.607104
171.184223	7113.609688	25.612122
171.218551	7123.059356	25.617139
171.526648	7133.861505	25.622157
172.020011	7146.131025	25.627175
172.186571	7146.610070	25.632192
172.253596	7160.910008	25.637210
172.206633	7166.110563	25.642227
171.967709	7182.163198	25.647245
172.564030	7194.328226	25.652263
172.900733	7212.816265	25.657280
173.209139	7218.295798	25.662298
173.320408	7216.494718	25.667315
173.413491	7239.500664	25.672333
173.415162	7241.236756	25.677351
173.265743	7256.031592	25.682368
173.465214	7274.212868	25.687386
173.780379	7271.745290	25.692404
173.841383	7292.091853	25.697421
173.740974	7305.025913	25.702439
174.440829	7312.732949	25.707456
174.362856	7336.261458	25.712474
175.040130	7338.377890	25.717492
174.786063	7362.865328	25.722509
175.019045	7363.715966	25.727527
175.414918	7376.736490	25.732544
175.139468	7388.305803	25.737562
175.570914	7395.073103	25.742580
175.603093	7414.818177	25.747597
176.312562	7410.808181	25.752615
176.334647	7413.260884	25.757632
176.175566	7433.241145	25.762650
176.691983	7440.332948	25.767668
176.658789	7451.188752	25.772685
177.115762	7465.162648	25.777703
177.193934	7466.166981	25.782720
177.467153	7488.920872	25.787738
177.992969	7490.928456	25.792756
177.572227	7499.451999	25.797773
177.804807	7509.464322	25.802791
177.983871	7516.429057	25.807808
178.513282	7519.815692	25.812826
179.177221	7534.495955	25.817844
178.736104	7545.857702	25.822861
179.227076	7558.020535	25.827879
179.282058	7547.581194	25.832896
179.325310	7556.104682	25.837914
179.844586	7558.353232	25.842932
179.434074	7577.034467	25.847949
179.679239	7578.801898	25.852967
180.299192	7582.729995	25.857984
179.898084	7603.805957	25.863002
180.348314	7590.801156	25.868020
180.805850	7612.661301	25.873037
180.904553	7623.152428	25.878055
180.748611	7626.567527	25.883072
181.002704	7631.897842	25.888090
180.872546	7642.213313	25.893108
181.244018	7652.873245	25.898125
181.541883	7659.330083	25.903143
182.067340	7668.289518	25.908160
182.006626	7678.070063	25.913178
182.333602	7676.636087	25.918196
182.562650	7696.296951	25.923213
182.527743	7709.719843	25.928231
182.790780	7704.021257	25.933248
182.744589	7723.734741	25.938266
183.380726	7727.227820	25.943284
183.392127	7733.489627	25.948301
183.425019	7733.822306	25.953319
183.601708	7748.973706	25.958336
183.427836	7762.970889	25.963354
183.589913	7766.866576	25.968372
184.031333	7775.141522	25.973389
184.572367	7790.226405	25.978407
184.624674	7800.346055	25.983424
184.623256	7804.832476	25.988442
184.832592	7818.302423	25.993460
184.413284	7835.921370	25.998477
185.024464	7848.217101	26.003495
185.521157	7860.322411	26.008512
185.138026	7862.342997	26.013530
185.700442	7874.507475	26.018548
185.742224	7890.898752	26.023565
186.151454	7890.102230	26.028583
186.648088	7909.184699	26.033600
186.689705	7924.407916	26.038618
186.800967	7911.929556	26.043636
186.969580	7918.179425	26.048653
187.148241	7932.393016	26.053671
187.169391	7934.577583	26.058688
187.241476	7946.907323	26.063706
187.582832	7958.711855	26.068724
187.932151	7976.008466	26.073741
187.970975	7963.194140	26.078759
188.259326	7975.420563	26.083776
188.022524	8000.256575	26.088794
188.273593	8000.946557	26.093812
188.564757	8021.469391	26.098829
188.945787	8028.892028	26.103847
189.449355	8031.124156	26.108864
189.220665	8053.439610	26.113882
188.941682	8054.474673	26.118900
189.536983	8066.858280	26.123917
189.737961	8087.846782	26.128935
189.769523	8090.411745	26.133952
189.684050	8100.231120	26.138970
190.229768	8121.828644	26.143988
190.571712	8136.537734	26.149005
190.694038	8148.411429	26.154023
191.058505	8163.053870	26.159040
191.224062	8169.427430	26.164058
191.692825	8177.455177	26.169076
191.771946	8188.139119	26.174093
191.527095	8199.079035	26.179111
191.737807	8206.171671	26.184128
192.058565	8218.279522	26.189146
192.421699	8229.809303	26.194164
192.842709	8244.461893	26.199181
192.965635	8245.500301	26.204199
193.327219	8243.214752	26.209216
193.154781	8263.965184	26.214234
193.664115	8268.608486	26.219252
194.072342	8274.562053	26.224269
193.828133	8275.645350	26.229287
194.123247	8276.719928	26.234304
193.996698	8297.576865	26.239322
194.272130	8302.888246	26.244340
194.650176	8316.518398	26.249357
194.531959	8327.350150	26.254375
194.852007	8335.319179	26.259392
194.651994	8345.889085	26.264410
194.774347	8374.208489	26.269428
195.278688	8380.064947	26.274445
195.529425	8403.713804	26.279463
195.655399	8401.872419	26.284480
195.417093	8426.914452	26.289498
195.975370	8433.924312	26.294516
196.093700	8462.793828	26.299533
195.852873	8472.527237	26.304551
196.293427	8491.802209	26.309568
196.444988	8513.326182	26.314586
196.886956	8532.559933	26.319604
197.218264	8548.215013	26.324621
197.440842	8561.576084	26.329639
197.854258	8578.159166	26.334656
197.702871	8595.995748	26.339674
197.727971	8609.346747	26.344692
198.336934	8614.811185	26.349709
198.647565	8637.557472	26.354727
198.996880	8636.268314	26.359744
198.987848	8654.483613	26.364762
199.151029	8664.981016	26.369780
199.205027	8673.440192	26.374797
199.544022	8678.659637	26.379815
200.343841	8691.396804	26.384832
200.542579	8705.535229	26.389850
200.312204	8702.493073	26.394868
200.874234	8695.601280	26.399885
200.757950	8703.844042	26.404903
201.030518	8705.266312	26.409920
200.912355	8719.410193	26.414938
200.836525	8726.639478	26.419956
201.177970	8738.315049	26.424973
201.337975	8757.953129	26.429991
201.624223	8765.217265	26.435008
201.782377	8783.201281	26.440026
202.130593	8794.190710	26.445044
202.626987	8804.200294	26.450061
202.487764	8806.912086	26.455079
202.740774	8820.038099	26.460096
202.647703	8825.764128	26.465114
203.006132	8851.673044	26.470132
203.707551	8852.396697	26.475149
203.607285	8869.085772	26.480167
203.896733	8887.090364	26.485184
203.830910	8890.797828	26.490202
204.050021	8906.609707	26.495220
204.992252	8917.945007	26.500237
204.653054	8926.052298	26.505255
204.829153	8934.284087	26.510272
205.028318	8952.934335	26.515290
205.293118	8960.694439	26.520308
205.547470	8972.642696	26.525325
205.041020	8978.960793	26.530343
205.246642	9001.405095	26.535360
205.620853	9030.030185	26.540378
205.898287	9041.011906	26.545396
206.139653	9054.515624	26.550413
206.244494	9088.957641	26.555431
206.725649	9094.978981	26.560448
206.668585	9107.727543	26.565466
206.604724	9128.714511	26.570484
207.425778	9139.096490	26.575501
207.383615	9156.528153	26.580519
207.570305	9173.358825	26.585536
207.849972	9190.162318	26.590554
208.099396	9207.261035	26.595572
208.641738	9223.508769	26.600589
208.545475	9245.896469	26.605607
208.990463	9246.294065	26.610624
209.053220	9256.520221	26.615642
209.226173	9279.408841	26.620660
209.983442	9294.858900	26.625677
209.685760	9302.385221	26.630695
210.187475	9315.715735	26.635712
210.362088	9332.286387	26.640730
210.316115	9337.629474	26.645748
210.653489	9343.345060	26.650765
210.861107	9362.452206	26.655783
211.288616	9367.402237	26.660800
211.370955	9381.092129	26.665818
211.626866	9386.299532	26.670836
212.293235	9395.281938	26.675853
212.285243	9402.633466	26.680871
212.398948	9405.002618	26.685888
212.706945	9419.140256	26.690906
212.767708	9442.141372	26.695924
212.972957	9433.429748	26.700941
212.992791	9451.748656	26.705959
213.659829	9461.545581	26.710976
213.625577	9461.440469	26.715994
213.571832	9475.685338	26.721012
214.030110	9488.514451	26.726029
214.133972	9492.792188	26.731047
214.246492	9490.037177	26.736064
214.688772	9512.372403	26.741082
214.617001	9518.755192	26.746100
215.016235	9529.506579	26.751117
215.108677	9537.988542	26.756135
215.232104	9545.338483	26.761152
215.366317	9549.965101	26.766170
215.689369	9566.563225	26.771188
215.976072	9574.673779	26.776205
216.034848	9593.081445	26.781223
216.255751	9604.909056	26.786240
216.918485	9623.765202	26.791258
216.740404	9629.842633	26.796276
217.199506	9647.890847	26.801293
217.119478	9659.007868	26.806311
217.150095	9667.329078	26.811328
217.372938	9677.634579	26.816346
217.411682	9705.047157	26.821364
217.702596	9717.807927	26.826381
217.659618	9736.866308	26.831399
218.165905	9756.302797	26.836416
218.330909	9777.541964	26.841434
218.777404	9792.750645	26.846452
219.051660	9801.987279	26.851469
219.042461	9829.104440	26.856487
219.326721	9832.899330	26.861504
219.996901	9860.450022	26.866522
220.094038	9861.262072	26.871540
220.469366	9885.572138	26.876557
220.380939	9897.631523	26.881575
220.754645	9911.048825	26.886592
220.914768	9918.273182	26.891610
221.197258	9954.106646	26.896628
221.530317	9949.211022	26.901645
221.355004	9974.377875	26.906663
221.736927	9987.645547	26.911680
221.900188	9993.309675	26.916698
221.974733	10010.603870	26.921716
222.280448	10026.336827	26.926733
222.850347	10042.394674	26.931751
223.094250	10061.149535	26.936768
223.595490	10057.506296	26.941786
223.518734	10075.354703	26.946804
224.133007	10076.363603	26.951821
224.224317	10086.904643	26.956839
224.669839	10110.086272	26.961856
224.785167	10112.439473	26.966874
224.777919	10111.660749	26.971892
225.334871	10119.565017	26.976909
225.022713	10133.718257	26.981927
225.088903	10141.803612	26.986944
225.618277	10161.593700	26.991962
225.640316	10175.505170	26.996980
225.931372	10193.362375	27.001997
226.245792	10200.698440	27.007015
226.210695	10211.916104	27.012032
226.789994	10226.978038	27.017050
226.669246	10238.550142	27.022068
226.614104	10255.154451	27.027085
227.312910	10273.490939	27.032103
227.812423	10286.819339	27.037120
227.938787	10293.452368	27.042138
228.049321	10309.894999	27.047156
228.293201	10316.070737	27.052173
228.327267	10341.063196	27.057191
228.589442	10339.784420	27.062208
228.647125	10343.892769	27.067226
228.765276	10367.596468	27.072244
229.108215	10378.527671	27.077261
229.071290	10397.472108	27.082279
229.522929	10421.082584	27.087296
229.978069	10429.981758	27.092314
230.191847	10440.453292	27.097332
230.344067	10449.576749	27.102349
230.658723	10457.740145	27.107367
230.750421	10473.510165	27.112384
231.387671	10483.454387	27.117402
231.451384	10502.282124	27.122420
231.479082	10506.376261	27.127437
231.821708	10518.371676	27.132455
231.837583	10526.190375	27.137472
232.431524	10551.205920	27.142490
232.371080	10564.060202	27.147508
232.947967	10578.197645	27.152525
232.997227	10585.872209	27.157543
233.157190	10592.582176	27.162560
233.393918	10608.149611	27.167578
233.672903	10631.534799	27.172596
233.617577	10644.220986	27.177613
234.150155	10663.647988	27.182631
234.111057	10683.723453	27.187648
234.265354	10699.411234	27.192666
234.424918	10725.988578	27.197684
234.782566	10742.013970	27.202701
234.930145	10754.857898	27.207719
235.060357	10777.584543	27.212736
235.294650	10795.883802	27.217754
235.535630	10821.374957	27.222772
236.072908	10833.343238	27.227789
236.437971	10856.396308	27.232807
236.528851	10870.382764	27.237824
236.713827	10894.127182	27.242842
237.059728	10905.377145	27.247860
237.337078	10920.689027	27.252877
237.852209	10942.042019	27.257895
237.608665	10955.392575	27.262912
238.119546	10977.961944	27.267930
238.512799	10988.989823	27.272948
238.379214	11003.298883	27.277965
239.241431	11011.970369	27.282983
239.144319	11036.453829	27.288000
239.800318	11041.520082	27.293018
239.899633	11055.776908	27.298036
239.996880	11067.744807	27.303053
240.070486	11083.076110	27.308071
240.404858	11101.969407	27.313088
240.791951	11110.759578	27.318106
240.852307	11122.597513	27.323124
240.634405	11150.857605	27.328141
240.782381	11171.270568	27.333159
240.877173	11189.219464	27.338176
241.665306	11209.611125	27.343194
241.435522	11232.495761	27.348212
241.906944	11247.452272	27.353229
242.515853	11267.875230	27.358247
242.673738	11281.971487	27.363264
242.965684	11303.246179	27.368282
242.788583	11312.671102	27.373300
243.369369	11330.645044	27.378317
243.253205	11343.739096	27.383335
243.925220	11367.363609	27.388352
244.278849	11379.894654	27.393370
244.805457	11395.041570	27.398388
245.106946	11396.806865	27.403405
245.101755	11403.697721	27.408423
245.456466	11427.779356	27.413440
245.565561	11430.411575	27.418458
245.770561	11439.407255	27.423476
246.170934	11446.297746	27.428493
246.267334	11451.609660	27.433511
246.392034	11475.307417	27.438528
246.697267	11485.016841	27.443546
247.007857	11494.295986	27.448564
246.585323	11511.457871	27.453581
247.057696	11529.035332	27.458599
247.339777	11550.984436	27.463616
247.718085	11565.374774	27.468634
247.983308	11582.479506	27.473652
248.257779	11600.583794	27.478669
248.407523	11622.187421	27.483687
248.733357	11642.333048	27.488704
248.749753	11652.327791	27.493722
249.134760	11677.535457	27.498740
249.335484	11693.807287	27.503757
249.620686	11702.878945	27.508775
250.045797	11732.084380	27.513792
250.272500	11733.678275	27.518810
250.477332	11757.376466	27.523828
250.487591	11778.787398	27.528845
251.152269	11788.639606	27.533863
251.075155	11815.325038	27.538880
251.205420	11839.256055	27.543898
251.176159	11859.577536	27.548916
251.392933	11876.746965	27.553933
252.162774	11903.173531	27.558951
252.485603	11929.771210	27.563968
252.488701	11934.652633	27.568986
252.659416	11957.386991	27.574004
253.231614	11979.742706	27.579021
253.348998	12004.370656	27.584039
253.690923	12026.418304	27.589056
254.095323	12038.357650	27.594074
254.112219	12060.206791	27.599092
254.445064	12086.919960	27.604109
254.746116	12106.732085	27.609127
255.106513	12125.906536	27.614144
255.523139	12138.254541	27.619162
255.615021	12159.040508	27.624180
256.097318	12178.884314	27.629197
255.889745	12198.665692	27.634215
256.171230	12216.264226	27.639232
256.472850	12235.372208	27.644250
256.926678	12246.596596	27.649268
256.608012	12278.590894	27.654285
257.226223	12294.005232	27.659303
257.622814	12322.221339	27.664320
257.725702	12333.210236	27.669338
257.937139	12353.570330	27.674356
258.068721	12377.233407	27.679373
258.461273	12391.675829	27.684391
258.889103	12414.626244	27.689408
259.382669	12435.946420	27.694426
259.696020	12454.958052	27.699444
259.534818	12475.193498	27.704461
259.946319	12492.667714	27.709479
260.022923	12517.874292	27.714496
260.477336	12541.872260	27.719514
260.702209	12554.651625	27.724532
260.628189	12576.427185	27.729549
261.341553	12596.326811	27.734567
261.196449	12606.858932	27.739584
261.500988	12632.573108	27.744602
261.938047	12645.650870	27.749620
261.843720	12663.258168	27.754637
262.102020	12695.535415	27.759655
262.663661	12708.208444	27.764672
263.071803	12730.486540	27.769690
263.201986	12743.457708	27.774708
263.418672	12757.403752	27.779725
263.716328	12777.393955	27.784743
263.663194	12800.249657	27.789760
263.992993	12826.875929	27.794778
264.120282	12846.921315	27.799796
264.208577	12867.389674	27.804813
265.089411	12891.772867	27.809831
265.026591	12917.715506	27.814848
265.381342	12927.654761	27.819866
265.789372	12948.881547	27.824884
266.053945	12966.480272	27.829901
266.843991	12987.543046	27.834919
267.068416	13003.161759	27.839936
267.331570	13025.743973	27.844954
267.929557	13028.966153	27.849972
267.954546	13055.204702	27.854989
268.539626	13063.888983	27.860007
268.309154	13083.160126	27.865024
268.703677	13090.061613	27.870042
269.225082	13104.181234	27.875060
269.490799	13118.644083	27.880077
269.586398	13132.653584	27.885095
269.884865	13156.613603	27.890112
269.886892	13174.136806	27.895130
270.347820	13188.796501	27.900148
270.396183	13207.070385	27.905165
270.377451	13221.543135	27.910183
270.634254	13242.481302	27.915200
270.910832	13267.367017	27.920218
271.397703	13284.785948	27.925236
271.322738	13318.515446	27.930253
271.716144	13331.306831	27.935271
271.862916	13350.108610	27.940288
272.043487	13371.380976	27.945306
272.815859	13389.058445	27.950324
272.453287	13420.104673	27.955341
273.223333	13442.437445	27.960359
273.223912	13468.642493	27.965376
273.649458	13497.086351	27.970394
273.918559	13516.364939	27.975412
274.360616	13534.286928	27.980429
274.688545	13556.764887	27.985447
274.804593	13575.094840	27.990464
275.304287	13597.100658	27.995482
275.875505	13605.054699	28.000500
275.654938	13631.070394	28.005517
276.553190	13643.650267	28.010535
276.694674	13657.823502	28.015552
277.160902	13669.845779	28.020570
277.528829	13680.263388	28.025588
277.599976	13704.828158	28.030605
277.990816	13708.420818	28.035623
278.070238	13738.722504	28.040640
278.354975	13755.027161	28.045658
278.501621	13755.449502	28.050676
278.727418	13775.853089	28.055693
278.527291	13797.836129	28.060711
278.955586	13819.092297	28.065728
279.003154	13834.676240	28.070746
279.562588	13855.292924	28.075764
280.168298	13881.075305	28.080781
280.480812	13893.046010	28.085799
280.188648	13910.960208	28.090816
280.532525	13936.489980	28.095834
281.092201	13943.561709	28.100852
280.986164	13968.931465	28.105869
281.409012	13991.448756	28.110887
281.719876	14011.652942	28.115904
281.879753	14039.832896	28.120922
282.410784	14058.344640	28.125940
282.322520	14078.166128	28.130957
282.824688	14096.549790	28.135975
283.075750	14130.933913	28.140992
283.065409	14153.481358	28.146010
283.553697	14168.557556	28.151028
283.935089	14196.854631	28.156045
284.195741	14206.705082	28.161063
284.616698	14239.019477	28.166080
284.470834	14264.537980	28.171098
285.058266	14286.192932	28.176116
285.185826	14315.799519	28.181133
285.503037	14329.535167	28.186151
286.127992	14345.367001	28.191168
286.307329	14376.421480	28.196186
286.807438	14394.016213	28.201204
286.766053	14411.364182	28.206221
287.362571	14433.504235	28.211239
287.503300	14448.988815	28.216256
287.618251	14473.601402	28.221274
288.079269	14491.597121	28.226292
288.256664	14531.040270	28.231309
288.455434	14553.662809	28.236327
289.107071	14576.366025	28.241344
288.779931	14603.132438	28.246362
289.323815	14618.907719	28.251380
289.748758	14651.417997	28.256397
290.384383	14662.438484	28.261415
290.560619	14689.631476	28.266432
290.708525	14721.411511	28.271450
291.281041	14730.294339	28.276468
291.382439	14758.228699	28.281485
292.017695	14780.284132	28.286503
292.139668	14797.287880	28.291520
292.248769	14815.604324	28.296538
292.750091	14832.520255	28.301556
293.188988	14849.136472	28.306573
293.041203	14870.986217	28.311591
293.630606	14894.324893	28.316608
293.619941	14918.376614	28.321626
294.186755	14929.679645	28.326644
294.399767	14959.618094	28.331661
294.629858	14977.473585	28.336679
294.903308	14996.901429	28.341696
294.927499	15023.247034	28.346714
295.407493	15041.044487	28.351732
295.609216	15073.205143	28.356749
295.525292	15095.051456	28.361767
295.827916	15129.211378	28.366784
295.723748	15159.398796	28.371802
296.922948	15188.750432	28.376820
297.088298	15210.084084	28.381837
297.347544	15230.281856	28.386855
297.754316	15255.667734	28.391872
298.259426	15287.752800	28.396890
298.562508	15304.933918	28.401908
298.872130	15317.177587	28.406925
298.816133	15341.028491	28.411943
299.169040	15357.355423	28.416960
299.837318	15384.996605	28.421978
300.224276	15396.659712	28.426996
300.403061	15405.702443	28.432013
300.747438	15418.092332	28.437031
301.030718	15439.309857	28.442048
300.854218	15453.856388	28.447066
301.636915	15472.336400	28.452084
301.798217	15500.704627	28.457101
301.868194	15518.415153	28.462119
302.021023	15537.369740	28.467136
302.390357	15564.571626	28.472154
303.223652	15588.381440	28.477172
303.212746	15604.127586	28.482189
303.261343	15619.810731	28.487207
303.858295	15651.904129	28.492224
303.782079	15671.829604	28.497242
304.627329	15690.814844	28.502260
304.579336	15707.871292	28.507277
304.831385	15741.841251	28.512295
305.172784	15762.990022	28.517312
305.705250	15789.696074	28.522330
306.429927	15819.672575	28.527348
306.128285	15832.890361	28.532365
306.081440	15853.222014	28.537383
306.747687	15879.190278	28.542400
306.960815	15900.997292	28.547418
307.243260	15938.263372	28.552436
307.748647	15952.700304	28.557453
308.090149	15987.370487	28.562471
308.349233	16009.852644	28.567488
308.127716	16034.482042	28.572506
308.746115	16065.075676	28.577524
308.866904	16092.614138	28.582541
309.013348	16130.350393	28.587559
309.657363	16157.510091	28.592576
309.790961	16184.506583	28.597594
310.017997	16215.796613	28.602612
310.448210	16240.434727	28.607629
310.852439	16276.750640	28.612647
311.386973	16299.995397	28.617664
311.604741	16328.393901	28.622682
311.891058	16347.855842	28.627700
312.487838	16384.422900	28.632717
312.325718	16406.194513	28.637735
312.997572	16431.922601	28.642752
313.416619	16465.832936	28.647770
313.498885	16487.481079	28.652788
314.118506	16516.953972	28.657805
314.500356	16540.819897	28.662823
315.089410	16555.133628	28.667840
315.437253	16582.507724	28.672858
315.814687	16593.993017	28.677876
316.093438	16613.598545	28.682893
316.390222	16627.572775	28.687911
316.541759	16642.706838	28.692928
316.732586	16673.775869	28.697946
316.636157	16697.896945	28.702964
317.066346	16723.255829	28.707981
317.086723	16749.522273	28.712999
317.879593	16769.653866	28.718016
318.342948	16805.415084	28.723034
318.309307	16833.626299	28.728052
318.694865	16852.880533	28.733069
319.086181	16876.265288	28.738087
319.556372	16884.214423	28.743104
320.256423	16911.685425	28.748122
320.502817	16930.434054	28.753140
320.955334	16954.235725	28.758157
321.123151	16964.891784	28.763175
321.003174	16977.165905	28.768192
321.309915	17008.962744	28.773210
321.568899	17029.541479	28.778228
321.713527	17051.212071	28.783245
322.018145	17074.613806	28.788263
322.585267	17094.474718	28.793280
322.685400	17124.977500	28.798298
322.913692	17152.289007	28.803316
323.263135	17175.848092	28.808333
323.608982	17199.957368	28.813351
324.179485	17225.282297	28.818368
324.653034	17247.760731	28.823386
324.595478	17280.505816	28.828404
325.039537	17298.737409	28.833421
325.219932	17328.185589	28.838439
325.486004	17351.315737	28.843456
325.817928	17381.416211	28.848474
326.148110	17412.003437	28.853492
326.787113	17433.660189	28.858509
326.679080	17459.546562	28.863527
327.360454	17487.128704	28.868544
327.644092	17523.358459	28.873562
327.850860	17535.859713	28.878580
328.388506	17568.196179	28.883597
328.487095	17604.796211	28.888615
329.049507	17621.897713	28.893632
329.570314	17653.838966	28.898650
329.815239	17672.335849	28.903668
330.522417	17699.775270	28.908685
330.608701	17723.906907	28.913703
331.008953	17740.616967	28.918720
331.247002	17773.297626	28.923738
331.162584	17796.533748	28.928756
331.774177	17828.890654	28.933773
331.950522	17853.589549	28.938791
332.487026	17871.087013	28.943808
332.820064	17900.272087	28.948826
332.723921	17923.592325	28.953844
333.575907	17953.372158	28.958861
333.579762	17977.535975	28.963879
334.348562	18006.078056	28.968896
334.258126	18036.631076	28.973914
334.552959	18061.854981	28.978932
335.018073	18087.538695	28.983949
335.458443	18117.484339	28.988967
335.769521	18146.660589	28.993984
336.450456	18173.043444	28.999002
336.607751	18202.844035	29.004020
337.064010	18227.171045	29.009037
337.202465	18261.643365	29.014055
337.637201	18270.287244	29.019072
337.445815	18311.539551	29.024090
337.863450	18342.171404	29.029108
338.786793	18367.966921	29.034125
338.727007	18398.092426	29.039143
339.319417	18417.420056	29.044160
339.513197	18447.777577	29.049178
339.537549	18478.749227	29.054196
340.345507	18502.332865	29.059213
340.295920	18539.280067	29.064231
340.802132	18558.678200	29.069248
340.590472	18585.599450	29.074266
341.062082	18616.968768	29.079284
341.424262	18647.919356	29.084301
341.666718	18687.676697	29.089319
342.164768	18722.977986	29.094336
342.693612	18754.565998	29.099354
342.768202	18789.023984	29.104372
343.246406	18808.717370	29.109389
343.281805	18845.462306	29.114407
343.903578	18869.757876	29.119424
344.354364	18902.065946	29.124442
344.127453	18941.903647	29.129460
345.068153	18968.417473	29.134477
344.861265	18994.359278	29.139495
345.325260	19020.619322	29.144512
345.623252	19063.995165	29.149530
345.885157	19105.165508	29.154548
346.689665	19129.274830	29.159565
347.193760	19168.802631	29.164583
347.082786	19196.050116	29.169600
347.438477	19226.926825	29.174618
347.984066	19262.783937	29.179636
348.543333	19289.939198	29.184653
348.793945	19331.623538	29.189671
349.090025	19358.472635	29.194688
349.421360	19386.194442	29.199706
350.070581	19422.515778	29.204724
350.566470	19434.530708	29.209741
350.500179	19468.228531	29.214759
351.069056	19497.612822	29.219776
352.219225	19523.911373	29.224794
352.533015	19536.359241	29.229812
353.214381	19564.146512	29.234829
353.289872	19563.585049	29.239847
353.568427	19593.343498	29.244864
353.975327	19621.293886	29.249882
353.949078	19648.219145	29.254900
354.216453	19663.681749	29.259917
354.660495	19699.454481	29.264935
354.700506	19729.124141	29.269952
355.228929	19753.909290	29.274970
355.067899	19780.078720	29.279988
355.518817	19811.750150	29.285005
355.972765	19858.799406	29.290023
356.339087	19887.312524	29.295040
356.691123	19921.034051	29.300058
357.098203	19943.709242	29.305076
357.439425	19966.476911	29.310093
357.802903	20001.112913	29.315111
358.200215	20042.042880	29.320128
358.749300	20066.041737	29.325146
358.753939	20106.862758	29.330164
359.664719	20129.907855	29.335181
359.650650	20163.769283	29.340199
359.947744	20199.129990	29.345216
360.286741	20220.356660	29.350234
360.637921	20257.307508	29.355252
361.029940	20293.184246	29.360269
361.517442	20327.175891	29.365287
361.845432	20357.559581	29.370304
362.456264	20383.924821	29.375322
362.512086	20418.420204	29.380340
363.018081	20451.448788	29.385357
363.356444	20478.242251	29.390375
363.790091	20506.764678	29.395392
364.257532	20532.015283	29.400410
364.933877	20557.283743	29.405428
365.293584	20576.125545	29.410445
365.784388	20604.607570	29.415463
365.642261	20629.397770	29.420480
366.676745	20657.428244	29.425498
366.805193	20689.240060	29.430516
367.181127	20714.865381	29.435533
367.134590	20730.055761	29.440551
367.630711	20758.631951	29.445568
367.970770	20781.621892	29.450586
368.311884	20803.790302	29.455604
368.556370	20828.842432	29.460621
368.893606	20851.479066	29.465639
368.820128	20880.030924	29.470656
369.238312	20909.706312	29.475674
369.487579	20941.708119	29.480692
369.752335	20971.673008	29.485709
370.359079	20996.618059	29.490727
370.329146	21043.771223	29.495744
371.130212	21075.402481	29.500762
371.527169	21123.101859	29.505780
371.757192	21143.430412	29.510797
372.272840	21177.785593	29.515815
372.320372	21213.863297	29.520832
373.013871	21255.261196	29.525850
373.038552	21292.448369	29.530868
373.525719	21311.738484	29.535885
374.400483	21351.433771	29.540903
374.717333	21391.709381	29.545920
374.934233	21416.210541	29.550938
375.528596	21465.092996	29.555956
375.503216	21505.283434	29.560973
375.648926	21531.742028	29.565991
375.721939	21569.598245	29.571008
376.490058	21593.419329	29.576026
377.086568	21636.305467	29.581044
377.584045	21671.656385	29.586061
378.082209	21696.631968	29.591079
378.878880	21730.046837	29.596096
379.741053	21757.025374	29.601114
380.007629	21788.741501	29.606132
380.244240	21805.992489	29.611149
380.792381	21835.225558	29.616167
380.704945	21865.101640	29.621184
381.499026	21884.849740	29.626202
381.733265	21923.357486	29.631220
381.887733	21939.382980	29.636237
382.560965	21965.430946	29.641255
382.525235	21999.949750	29.646272
383.185192	22022.107499	29.651290
383.048362	22062.651422	29.656308
383.367937	22088.931874	29.661325
383.541666	22114.249470	29.666343
384.087320	22152.550910	29.671360
384.424016	22190.259590	29.676378
384.430648	22235.033977	29.681396
385.221053	22272.671745	29.686413
385.500669	22313.915532	29.691431
385.425092	22350.728624	29.696448
386.284868	22392.854809	29.701466
386.969981	22425.188838	29.706484
387.119282	22466.137407	29.711501
387.780709	22499.966536	29.716519
387.892830	22541.091696	29.721536
388.409286	22571.777857	29.726554
389.068050	22608.583823	29.731572
389.419841	22637.134788	29.736589
389.559406	22665.826460	29.741607
390.297662	22703.605914	29.746624
390.522442	22729.535561	29.751642
391.042207	22769.700040	29.756660
391.209005	22798.387637	29.761677
391.512690	22832.462941	29.766695
391.732351	22864.990656	29.771712
392.738314	22899.967121	29.776730
392.816669	22944.523340	29.781748
392.664079	22965.975303	29.786765
393.689169	23006.231722	29.791783
393.567263	23043.716858	29.796800
394.304319	23060.125934	29.801818
394.348142	23105.136579	29.806836
394.768969	23149.582740	29.811853
395.382388	23177.423670	29.816871
395.613962	23208.433482	29.821888
396.311185	23235.269256	29.826906
396.635560	23277.083074	29.831924
396.751645	23317.583616	29.836941
397.603026	23339.295787	29.841959
397.831771	23380.044215	29.846976
398.276909	23415.766635	29.851994
398.562829	23456.234536	29.857012
398.552540	23485.753405	29.862029
399.078210	23520.799877	29.867047
399.514678	23565.933316	29.872064
399.754821	23604.689843	29.877082
400.429771	23640.294517	29.882100
400.682323	23679.965546	29.887117
401.230956	23711.122374	29.892135
401.411923	23762.097422	29.897152
401.947893	23797.357623	29.902170
402.445096	23838.753746	29.907188
402.544281	23889.261656	29.912205
402.813877	23928.728289	29.917223
403.080113	23976.631939	29.922240
403.834058	24021.520776	29.927258
404.460173	24066.056890	29.932276
404.744343	24109.401733	29.937293
405.163865	24148.143854	29.942311
405.557341	24191.806685	29.947328
405.977705	24233.158784	29.952346
406.435331	24278.037737	29.957364
407.087859	24304.502781	29.962381
407.141300	24345.937865	29.967399
407.573868	24403.415848	29.972416
408.020294	24438.754401	29.977434
408.761888	24483.083768	29.982452
409.038128	24523.005539	29.987469
409.345493	24560.287242	29.992487
409.985589	24600.057379	29.997504
410.445918	24641.909630	30.002522
410.948016	24689.215591	30.007540
411.153477	24721.242979	30.012557
411.702902	24757.956284	30.017575
411.938409	24795.938523	30.022592
412.995269	24821.759509	30.027610
413.232888	24858.951577	30.032628
413.453269	24896.310725	30.037645
414.304450	24922.435805	30.042663
414.418128	24965.847121	30.047680
414.942147	24995.707941	30.052698
415.451001	25023.093842	30.057716
416.059279	25054.919632	30.062733
416.407035	25074.702899	30.067751
416.744378	25110.811773	30.072768
417.217922	25146.640267	30.077786
417.543948	25181.152136	30.082804
417.548136	25222.034278	30.087821
417.920829	25247.703867	30.092839
418.159467	25280.940353	30.097856
418.902364	25314.597176	30.102874
419.142799	25366.761430	30.107892
419.496895	25406.900275	30.112909
420.384337	25445.261933	30.117927
420.484677	25483.405678	30.122944
420.792661	25517.130963	30.127962
420.816855	25549.308139	30.132980
421.290879	25594.705695	30.137997
422.102702	25623.062465	30.143015
422.150484	25667.465201	30.148032
422.534624	25703.498287	30.153050
423.127210	25734.803054	30.158068
423.290232	25774.536482	30.163085
424.232227	25817.270048	30.168103
424.311043	25859.222509	30.173120
424.510121	25899.329734	30.178138
425.221006	25936.588700	30.183156
425.175796	25981.910457	30.188173
426.171033	26017.469182	30.193191
426.566208	26052.679556	30.198208
426.788289	26093.965416	30.203226
427.456144	26136.666758	30.208244
427.764371	26181.725038	30.213261
428.648225	26211.044649	30.218279
428.598769	26263.142862	30.223296
428.944537	26300.244805	30.228314
429.341522	26338.280495	30.233332
429.768396	26388.168208	30.238349
430.452544	26430.045995	30.243367
430.887467	26478.851920	30.248384
430.968574	26515.584899	30.253402
431.695911	26557.734275	30.258420
431.884881	26604.777764	30.263437
431.937634	26651.254914	30.268455
432.474713	26699.704075	30.273472
432.766656	26746.251423	30.278490
434.010501	26790.791610	30.283508
434.477888	26842.671307	30.288525
435.179148	26883.814197	30.293543
435.256535	26927.993845	30.298560
435.989072	26964.492873	30.303578
436.418695	26992.614376	30.308596
436.725463	27044.481826	30.313613
437.529526	27080.129249	30.318631
437.789416	27117.024923	30.323648
438.194992	27158.935209	30.328666
438.826177	27193.352149	30.333684
439.074164	27228.107267	30.338701
439.448107	27269.807842	30.343719
439.870401	27314.319852	30.348736
440.097913	27349.280638	30.353754
440.387522	27394.730075	30.358772
441.267562	27439.518287	30.363789
441.856716	27482.955327	30.368807
442.370071	27531.296418	30.373824
442.678965	27577.432178	30.378842
443.136263	27602.137100	30.383860
443.664208	27648.971895	30.388877
443.945555	27692.299581	30.393895
444.304589	27724.592091	30.398912
444.536446	27760.096472	30.403930
445.430360	27796.906709	30.408948
445.229534	27847.408289	30.413965
445.681504	27891.145795	30.418983
446.111749	27943.805233	30.424000
446.546027	27985.611593	30.429018
447.257201	28028.038339	30.434036
447.405089	28079.642556	30.439053
447.817668	28123.032769	30.444071
448.335878	28168.991704	30.449088
448.929827	28214.249918	30.454106
449.555084	28256.090126	30.459124
449.668239	28308.319793	30.464141
450.164437	28348.126155	30.469159
450.675536	28385.800156	30.474176
451.158441	28425.387523	30.479194
451.712301	28459.047575	30.484212
451.728102	28504.163118	30.489229
452.584313	28543.098084	30.494247
452.992882	28583.165142	30.499264
453.432073	28635.768072	30.504282
454.374017	28669.260229	30.509300
454.536443	28711.104331	30.514317
455.118703	28734.526874	30.519335
455.921164	28765.601171	30.524352
456.292273	28813.468223	30.529370
456.944602	28835.103728	30.534388
457.423114	28877.720382	30.539405
457.963386	28902.559263	30.544423
458.304691	28939.906906	30.549440
458.481596	28963.311029	30.554458
459.305857	29005.722091	30.559476
459.556688	29038.065227	30.564493
460.265794	29073.787900	30.569511
460.677240	29107.490287	30.574528
461.211761	29133.341711	30.579546
461.403460	29166.199992	30.584564
461.520432	29202.875296	30.589581
461.967021	29252.520403	30.594599
462.432269	29291.663414	30.599616
462.600090	29339.677313	30.604634
463.292289	29373.203419	30.609652
463.659013	29433.518834	30.614669
464.169374	29457.086208	30.619687
464.602770	29511.468523	30.624704
464.672623	29559.163258	30.629722
465.495870	29608.807119	30.634740
466.045206	29656.319518	30.639757
466.726593	29694.550798	30.644775
466.987718	29741.716622	30.649792
467.440781	29791.526366	30.654810
467.643981	29828.638084	30.659828
467.980016	29888.574042	30.664845
468.504197	29936.862219	30.669863
468.646024	29990.330634	30.674880
468.948820	30042.320076	30.679898
469.416656	30097.558238	30.684916
469.836239	30159.428860	30.689933
470.474638	30211.163879	30.694951
471.230270	30256.236913	30.699968
471.729806	30310.933365	30.704986
472.448213	30363.756154	30.710004
473.127704	30415.478927	30.715021
474.024887	30467.907339	30.720039
474.576344	30503.505472	30.725056
474.845925	30548.370809	30.730074
475.338595	30582.499066	30.735092
476.170412	30635.905326	30.740109
476.561955	30669.373168	30.745127
476.717825	30705.924939	30.750144
476.926418	30750.503156	30.755162
477.607527	30797.308495	30.760180
477.834511	30844.362072	30.765197
478.194718	30893.961440	30.770215
479.423152	30928.531322	30.775232
479.761019	30976.914326	30.780250
480.091644	31010.607194	30.785268
480.591155	31057.036981	30.790285
480.536730	31112.625160	30.795303
481.040449	31157.720651	30.800320
481.357731	31208.667681	30.805338
482.061717	31237.851997	30.810356
482.467034	31290.346888	30.815373
483.162959	31331.158164	30.820391
483.508538	31364.558466	30.825408
484.264422	31414.166641	30.830426
484.686393	31453.099264	30.835444
485.047840	31486.946120	30.840461
485.026012	31536.543642	30.845479
485.941046	31574.191810	30.850496
486.240155	31634.043772	30.855514
486.605133	31667.915656	30.860532
487.302865	31714.796322	30.865549
487.648376	31766.796038	30.870567
487.983382	31813.423970	30.875584
488.682042	31868.542188	30.880602
489.126374	31920.906122	30.885620
490.211095	31972.107808	30.890637
490.424077	32009.228215	30.895655
490.690725	32053.357598	30.900672
490.692222	32112.296615	30.905690
491.443752	32155.439910	30.910708
492.146156	32218.113184	30.915725
492.873475	32280.302273	30.920743
493.013410	32319.792769	30.925760
493.115854	32378.489134	30.930778
494.141452	32424.630945	30.935796
494.157501	32476.134014	30.940813
494.852364	32530.097642	30.945831
495.932779	32578.823249	30.950848
496.061890	32642.112319	30.955866
496.574728	32684.073930	30.960884
497.086892	32741.973777	30.965901
497.476061	32808.168721	30.970919
497.981280	32856.795403	30.975936
498.257418	32908.998490	30.980954
499.012404	32969.105301	30.985972
499.660700	33029.785348	30.990989
499.739072	33090.725536	30.996007
500.753088	33131.572702	31.001024
500.797510	33193.694442	31.006042
501.566077	33249.829556	31.011060
501.895971	33299.224430	31.016077
502.375684	33362.631459	31.021095
502.648808	33422.378801	31.026112
503.366499	33485.243140	31.031130
503.839813	33543.220828	31.036148
504.533919	33598.559276	31.041165
504.660658	33660.384992	31.046183
505.464539	33710.288252	31.051200
505.903309	33776.864145	31.056218
506.334957	33836.448740	31.061236
506.949326	33897.882655	31.066253
507.542555	33965.560350	31.071271
508.062216	34018.183266	31.076288
508.297601	34078.551662	31.081306
508.828150	34138.153231	31.086324
509.803922	34198.089879	31.091341
510.252154	34247.696053	31.096359
510.988302	34293.014796	31.101376
511.418774	34350.685286	31.106394
512.079934	34396.667225	31.111412
512.575205	34455.187725	31.116429
512.784074	34503.807725	31.121447
513.405752	34553.671970	31.126464
513.964756	34612.176601	31.131482
514.996421	34661.648108	31.136500
515.897540	34699.746666	31.141517
516.263583	34748.127638	31.146535
516.665033	34790.920204	31.151552
517.146745	34813.505458	31.156570
517.596260	34853.287323	31.161588
517.893395	34891.449212	31.166605
518.380337	34945.634961	31.171623
519.170696	34980.861866	31.176640
519.443001	35031.787282	31.181658
519.650106	35089.102754	31.186676
519.841161	35134.318992	31.191693
520.728535	35185.363418	31.196711
521.154504	35223.764963	31.201728
521.741181	35276.747241	31.206746
522.192301	35331.793175	31.211764
522.831610	35379.930456	31.216781
522.693056	35432.976128	31.221799
523.238828	35484.100068	31.226816
523.718975	35546.754828	31.231834
524.669697	35619.187263	31.236852
524.776694	35677.620198	31.241869
525.464911	35741.248299	31.246887
525.947520	35798.560470	31.251904
526.706370	35851.384430	31.256922
527.005329	35915.111955	31.261940
527.903062	35969.539483	31.266957
528.368725	36040.588692	31.271975
528.701407	36088.370923	31.276992
529.574317	36141.822696	31.282010
530.034401	36207.302658	31.287028
530.704899	36258.345690	31.292045
530.803086	36325.823908	31.297063
531.172408	36375.004789	31.302080
532.105042	36433.481207	31.307098
532.627981	36499.002804	31.312116
533.302827	36549.521023	31.317133
533.691561	36615.247370	31.322151
534.216457	36670.854302	31.327168
534.997830	36725.049051	31.332186
535.084541	36790.595601	31.337204
535.868574	36842.052232	31.342221
536.232601	36906.992927	31.347239
536.825961	36966.447151	31.352256
537.629332	37035.461235	31.357274
538.054065	37091.862725	31.362292
538.886896	37139.303386	31.367309
539.274986	37210.634215	31.372327
539.577398	37261.060682	31.377344
540.633874	37302.826151	31.382362
541.212404	37370.510658	31.387380
541.452427	37425.987109	31.392397
541.983683	37490.808526	31.397415
542.711498	37538.456224	31.402432
543.413518	37602.511379	31.407450
543.362822	37653.626427	31.412468
544.556410	37685.575952	31.417485
545.361303	37741.742547	31.422503
546.210735	37798.534675	31.427520
546.509647	37847.401133	31.432538
546.826585	37901.418651	31.437556
547.708934	37947.323020	31.442573
547.925408	38002.279780	31.447591
548.334381	38058.920252	31.452608
548.647220	38105.261958	31.457626
549.453906	38159.595488	31.462644
550.166149	38205.830590	31.467661
550.581423	38266.618993	31.472679
550.987391	38314.261904	31.477696
551.842036	38358.963650	31.482714
552.027923	38406.862567	31.487732
552.917682	38443.578360	31.492749
553.080988	38505.311202	31.497767
553.870931	38554.115003	31.502784
554.240805	38604.432867	31.507802
554.614551	38655.161294	31.512820
555.208039	38704.609618	31.517837
555.674945	38767.307480	31.522855
556.241931	38818.265304	31.527872
556.981861	38878.277329	31.532890
556.819306	38934.649145	31.537908
557.573034	38981.233551	31.542925
557.692973	39057.178387	31.547943
558.529643	39113.855820	31.552960
559.017665	39174.685973	31.557978
559.392775	39248.030283	31.562996
560.622291	39300.605616	31.568013
561.182884	39351.502455	31.573031
562.112172	39414.401705	31.578048
562.777068	39471.733064	31.583066
562.917881	39525.681035	31.588084
563.664773	39578.263065	31.593101
564.252809	39637.814023	31.598119
564.963134	39691.862935	31.603136
565.333313	39745.908337	31.608154
565.780220	39800.586925	31.613172
567.117419	39858.066976	31.618189
567.166936	39917.348886	31.623207
567.497757	39976.295984	31.628224
568.081951	40030.251654	31.633242
568.538241	40097.938545	31.638260
569.360067	40143.629381	31.643277
569.595876	40210.617533	31.648295
570.272171	40273.963651	31.653312
570.915913	40332.027888	31.658330
571.379550	40409.074642	31.663348
572.043402	40466.415108	31.668365
572.730735	40528.735684	31.673383
572.970042	40587.452113	31.678400
573.515111	40657.884286	31.683418
574.310908	40719.619219	31.688436
575.129603	40781.066138	31.693453
575.269629	40846.053727	31.698471
575.630846	40909.052589	31.703488
576.680338	40974.208021	31.708506
577.004375	41048.047049	31.713524
577.838474	41107.468612	31.718541
578.465113	41177.042186	31.723559
578.778230	41239.246306	31.728576
579.464519	41294.264292	31.733594
580.074680	41377.919725	31.738612
580.589834	41437.828537	31.743629
581.229485	41507.154457	31.748647
581.581124	41579.890453	31.753664
581.826576	41649.518900	31.758682
582.561318	41714.536086	31.763700
583.237568	41785.368769	31.768717
584.117519	41846.720533	31.773735
584.520991	41915.389003	31.778752
585.090750	41978.149550	31.783770
585.693396	42057.558459	31.788788
586.669213	42116.505167	31.793805
587.167909	42188.764751	31.798823
587.505240	42255.370075	31.803840
588.517721	42327.290324	31.808858
589.033274	42390.743628	31.813876
589.592736	42454.379986	31.818893
590.204410	42512.328515	31.823911
590.429796	42590.780104	31.828928
591.094901	42639.745417	31.833946
591.348600	42697.630321	31.838964
592.096482	42766.494174	31.843981
592.744057	42832.502367	31.848999
593.096636	42902.548093	31.854016
593.648836	42960.987819	31.859034
594.017986	43034.813784	31.864052
594.516393	43102.541280	31.869069
595.045981	43178.739830	31.874087
595.539924	43252.395170	31.879104
596.584250	43320.815832	31.884122
596.802792	43402.668005	31.889140
597.335655	43475.337578	31.894157
597.582134	43545.104661	31.899175
598.676552	43634.423498	31.904192
599.246257	43708.973005	31.909210
600.103738	43792.668420	31.914228
600.530041	43865.975843	31.919245
601.222976	43946.073169	31.924263
601.498987	44022.042331	31.929280
602.207708	44094.186675	31.934298
602.455477	44178.991102	31.939316
603.390459	44260.114325	31.944333
604.177658	44337.592198	31.949351
604.773656	44420.552887	31.954368
605.974579	44485.840449	31.959386
606.617130	44560.280185	31.964404
607.412984	44635.929649	31.969421
607.848467	44695.208209	31.974439
608.662230	44770.684533	31.979456
609.446147	44836.310432	31.984474
609.860486	44909.553571	31.989492
610.600954	44983.523932	31.994509
611.207285	45041.138300	31.999527
611.270914	45111.729625	32.004544
612.138722	45192.487210	32.009562
612.981798	45260.464589	32.014580
613.585362	45327.923016	32.019597
614.403883	45405.956351	32.024615
614.945609	45469.591451	32.029632
615.823518	45533.186733	32.034650
616.142607	45602.044266	32.039668
616.578242	45674.799475	32.044685
617.663742	45748.262858	32.049703
618.240471	45814.468094	32.054720
618.697751	45877.004211	32.059738
619.701353	45942.984823	32.064756
620.580488	46002.456719	32.069773
621.454576	46057.431785	32.074791
622.297187	46120.844478	32.079808
623.075144	46166.738074	32.084826
623.424122	46218.348092	32.089844
623.943987	46279.388907	32.094861
624.812408	46331.563091	32.099879
625.040140	46403.271456	32.104896
625.791995	46451.586284	32.109914
625.973359	46516.425803	32.114932
626.528475	46584.262496	32.119949
627.322336	46643.034584	32.124967
627.629456	46709.253040	32.129984
628.255246	46774.434896	32.135002
628.520974	46845.297328	32.140020
629.078735	46912.154028	32.145037
629.734983	46985.125633	32.150055
629.888875	47073.574285	32.155072
630.261041	47138.088366	32.160090
630.970161	47222.540997	32.165108
631.819855	47298.494639	32.170125
632.296503	47367.876940	32.175143
632.805453	47447.794132	32.180160
633.627141	47514.086182	32.185178
633.594799	47595.879036	32.190196
633.977340	47677.442721	32.195213
634.758118	47758.583721	32.200231
635.203946	47852.265950	32.205248
636.001670	47938.168781	32.210266
636.494416	48022.607658	32.215284
637.068539	48123.343974	32.220301
638.076561	48203.445046	32.225319
638.472103	48286.078064	32.230336
639.448698	48367.646081	32.235354
640.198639	48456.835544	32.240372
640.596461	48543.935755	32.245389
641.666507	48609.091254	32.250407
642.538329	48686.406298	32.255424
643.350288	48767.520696	32.260442
644.175253	48845.817935	32.265460
645.104564	48934.848309	32.270477
646.251260	48993.178950	32.275495
646.409586	49072.365890	32.280512
647.282117	49133.707108	32.285530
647.486912	49210.989195	32.290548
648.072205	49289.888577	32.295565
649.046704	49353.422496	32.300583
650.166877	49419.331680	32.305600
651.145954	49475.019840	32.310618
652.125014	49541.489264	32.315636
652.867324	49600.099899	32.320653
653.822655	49653.495521	32.325671
654.779069	49709.459859	32.330688
655.083850	49759.414490	32.335706
655.252267	49820.152861	32.340724
656.254549	49878.008535	32.345741
656.970459	49934.915855	32.350759
656.951485	49992.982373	32.355776
657.393652	50056.740801	32.360794
658.045281	50136.581762	32.365812
658.429537	50207.954872	32.370829
659.139232	50277.309491	32.375847
659.521845	50351.543177	32.380864
660.497226	50419.875903	32.385882
661.207624	50491.274739	32.390900
661.289670	50570.605316	32.395917
662.191983	50650.680865	32.400935
662.322099	50734.787883	32.405952
662.844434	50814.303432	32.410970
663.518796	50901.109833	32.415988
663.902009	50997.782203	32.421005
664.780083	51070.966189	32.426023
665.155944	51163.881943	32.431040
665.937247	51252.830554	32.436058
666.824108	51346.679401	32.441076
667.619231	51429.906515	32.446093
668.573792	51501.744784	32.451111
669.422941	51595.031065	32.456128
670.225563	51670.582593	32.461146
670.927622	51743.277404	32.466164
671.563283	51827.239598	32.471181
672.210091	51897.501099	32.476199
672.639906	51973.156285	32.481216
673.156318	52058.998308	32.486234
674.020907	52140.774381	32.491252
674.753320	52229.234494	32.496269
675.022510	52305.346193	32.501287
675.703518	52399.136601	32.506304
676.739627	52471.161248	32.511322
677.371326	52547.197979	32.516340
678.013328	52630.978564	32.521357
678.730188	52702.047799	32.526375
679.342004	52778.354163	32.531392
680.080939	52852.097071	32.536410
680.292419	52937.996400	32.541428
681.119145	53024.274284	32.546445
681.531704	53087.672306	32.551463
682.202193	53179.790587	32.556480
682.865717	53260.931299	32.561498
683.606615	53340.225058	32.566516
683.916688	53439.393224	32.571533
684.778317	53517.314478	32.576551
685.228530	53618.378845	32.581568
685.918764	53696.371829	32.586586
687.081359	53789.124174	32.591604
687.981920	53875.969478	32.596621
688.998038	53950.317891	32.601639
689.601142	54043.690421	32.606656
689.860929	54126.200944	32.611674
690.966190	54212.123152	32.616692
691.444714	54291.815581	32.621709
692.371932	54376.070299	32.626727
692.611479	54480.601265	32.631744
693.587659	54566.158949	32.636762
694.169914	54661.315438	32.641780
694.626261	54744.575718	32.646797
695.375587	54841.042048	32.651815
695.962313	54934.142205	32.656832
696.545468	55030.091083	32.661850
697.435711	55114.044122	32.666868
697.965870	55216.349497	32.671885
699.058850	55303.309129	32.676903
699.832694	55402.748299	32.681920
700.222610	55490.046543	32.686938
700.886112	55578.669237	32.691956
701.298000	55685.596028	32.696973
702.056219	55784.950640	32.701991
702.861780	55877.678469	32.707008
703.472951	55979.923804	32.712026
704.821416	56067.548700	32.717044
705.823267	56171.480398	32.722061
706.656139	56262.882739	32.727079
707.211208	56344.202875	32.732096
707.763694	56426.827425	32.737114
708.761572	56523.274295	32.742132
709.489350	56619.143624	32.747149
710.052954	56702.311665	32.752167
710.894318	56788.366778	32.757184
711.985357	56879.794331	32.762202
712.824036	56954.914079	32.767220
713.053088	57049.572123	32.772237
713.934319	57125.078135	32.777255
714.799546	57213.700605	32.782272
715.265849	57303.360546	32.787290
716.446023	57379.371168	32.792308
717.295119	57459.902207	32.797325
718.013655	57539.099534	32.802343
718.342715	57618.896088	32.807360
718.839546	57716.248996	32.812378
719.747765	57788.524997	32.817396
720.208814	57877.979034	32.822413
721.123447	57964.931952	32.827431
721.759691	58055.390871	32.832448
722.382482	58133.668414	32.837466
722.959887	58224.972642	32.842484
722.943231	58325.661664	32.847501
724.100448	58403.869047	32.852519
724.728032	58499.641286	32.857536
724.979622	58589.206702	32.862554
726.152071	58673.919169	32.867572
726.641979	58767.979772	32.872589
727.178494	58860.761221	32.877607
728.227731	58944.487546	32.882624
728.841572	59039.422245	32.887642
729.622660	59130.216938	32.892660
730.203010	59233.721475	32.897677
730.657654	59322.726110	32.902695
731.591245	59411.390224	32.907712
732.597875	59512.936643	32.912730
732.932073	59610.436544	32.917748
733.868633	59718.533309	32.922765
734.747797	59801.384070	32.927783
735.897632	59905.245350	32.932800
736.899008	59991.141199	32.937818
737.730287	60070.981087	32.942836
738.572728	60157.718949	32.947853
739.340634	60243.601606	32.952871
740.776542	60329.569851	32.957888
741.205402	60418.645810	32.962906
742.038153	60495.151021	32.967924
743.100687	60566.202104	32.972941
743.672039	60643.539948	32.977959
744.362720	60729.252831	32.982976
744.879211	60808.916540	32.987994
745.757549	60893.524519	32.993012
746.180489	60977.710363	32.998029
747.026411	61067.444979	33.003047
748.289858	61147.879015	33.008064
748.819342	61243.253247	33.013082
749.588605	61317.916252	33.018100
750.247439	61401.636158	33.023117
750.973729	61479.768947	33.028135
751.584564	61570.561357	33.033152
751.989976	61661.905343	33.038170
752.901443	61741.332966	33.043188
753.210128	61842.251349	33.048205
753.863921	61927.917201	33.053223
754.921616	62030.263634	33.058240
755.826653	62112.269870	33.063258
756.283037	62230.581316	33.068276
756.966292	62320.073748	33.073293
758.223270	62401.981516	33.078311
758.940299	62493.115176	33.083328
759.945621	62581.254056	33.088346
760.730294	62672.884214	33.093364
761.063707	62767.769590	33.098381
761.734854	62853.587848	33.103399
762.886520	62951.549006	33.108416
763.588598	63048.131265	33.113434
764.540664	63130.690582	33.118452
765.997690	63208.758696	33.123469
767.373222	63263.359706	33.128487
768.674679	63329.494109	33.133504
769.158803	63413.020252	33.138522
769.678443	63471.490809	33.143540
770.126616	63552.161603	33.148557
770.864435	63631.027374	33.153575
771.917300	63695.536710	33.158592
772.268004	63780.376431	33.163610
772.901039	63844.534068	33.168628
773.742271	63934.874864	33.173645
774.189602	64010.375047	33.178663
774.840313	64093.763419	33.183680
775.394169	64193.405754	33.188698
775.991463	64274.068180	33.193716
776.442290	64352.898861	33.198733
776.607209	64446.671100	33.203751
777.584261	64529.237446	33.208768
777.648867	64627.267764	33.213786
778.385711	64719.318079	33.218804
779.281356	64827.646102	33.223821
780.092422	64927.675238	33.228839
780.777833	65030.655710	33.233856
780.795215	65146.650214	33.238874
781.691109	65251.497938	33.243892
782.539421	65365.147449	33.248909
783.468210	65490.592429	33.253927
784.393461	65599.058405	33.258944
785.324136	65710.866863	33.263962
785.969626	65809.937748	33.268980
787.288679	65913.765936	33.273997
788.668322	66018.040912	33.279015
789.087000	66119.554403	33.284032
789.483698	66225.066802	33.289050
790.872266	66331.722242	33.294068
791.540019	66430.139929	33.299085
792.153403	66544.477303	33.304103
793.296458	66651.881646	33.309120
794.235762	66768.011429	33.314138
794.770335	66871.535829	33.319156
795.481226	66966.213255	33.324173
795.833515	67076.345458	33.329191
797.217227	67188.083124	33.334208
797.711563	67297.326610	33.339226
798.645188	67410.250085	33.344244
799.410251	67525.967378	33.349261
800.110085	67642.797117	33.354279
801.265654	67741.175115	33.359296
801.910219	67859.401134	33.364314
802.797070	67967.933839	33.369332
803.470033	68078.368368	33.374349
804.156571	68195.177370	33.379367
805.303622	68303.765722	33.384384
805.762613	68405.959460	33.389402
806.404091	68523.087262	33.394420
807.765158	68632.143701	33.399437
808.128874	68750.417781	33.404455
809.116082	68867.163742	33.409472
809.673787	68993.279190	33.414490
810.279585	69105.298960	33.419508
811.423748	69230.057320	33.424525
811.660735	69351.678315	33.429543
812.877731	69475.191691	33.434560
813.437764	69593.666827	33.439578
813.935581	69722.688983	33.444596
815.017055	69830.616459	33.449613
816.348350	69956.799077	33.454631
817.492693	70073.107924	33.459648
818.216829	70191.762713	33.464666
819.114235	70299.549982	33.469684
820.197521	70409.930179	33.474701
821.035695	70524.883200	33.479719
821.815880	70630.752485	33.484736
822.795256	70750.851623	33.489754
823.529306	70862.187617	33.494772
824.742999	70968.826268	33.499789
824.996369	71080.504422	33.504807
826.169063	71184.490718	33.509824
826.980313	71289.737209	33.514842
827.360200	71398.534587	33.519860
828.286536	71520.330015	33.524877
829.285870	71626.371639	33.529895
830.338025	71724.350275	33.534912
831.162680	71831.192661	33.539930
831.981711	71919.202886	33.544948
833.349482	72015.663995	33.549965
833.753174	72125.879175	33.554983
834.949310	72205.446738	33.560000
835.597201	72303.516157	33.565018
836.375327	72397.727858	33.570036
837.453175	72494.261444	33.575053
838.338897	72599.387502	33.580071
838.833602	72686.209822	33.585088
839.561417	72792.095985	33.590106
840.036331	72893.576448	33.595124
841.261845	72992.267253	33.600141
841.793803	73114.638408	33.605159
842.454536	73215.014390	33.610176
843.053668	73321.682772	33.615194
843.766058	73430.512420	33.620212
845.063011	73546.280708	33.625229
845.780904	73660.455562	33.630247
846.628096	73758.904458	33.635264
848.045078	73858.607126	33.640282
848.770182	73981.167334	33.645300
849.649868	74080.422974	33.650317
850.393799	74201.879264	33.655335
851.356532	74308.722643	33.660352
852.319749	74415.465040	33.665370
853.097016	74528.734968	33.670388
853.711847	74635.456791	33.675405
854.206284	74754.281972	33.680423
855.142554	74871.961812	33.685440
856.342002	74981.722167	33.690458
856.844159	75093.720197	33.695476
857.646489	75210.637140	33.700493
858.709906	75333.707882	33.705511
859.144712	75458.765012	33.710528
859.970094	75585.914975	33.715546
861.049758	75716.927218	33.720564
861.904245	75835.320756	33.725581
862.836110	75952.435964	33.730599
863.989259	76065.906826	33.735616
865.245286	76182.566912	33.740634
865.842716	76299.241953	33.745652
866.954110	76408.135156	33.750669
867.722192	76529.154759	33.755687
868.799379	76638.130244	33.760704
869.565239	76743.835981	33.765722
869.884739	76870.855817	33.770740
871.279680	76981.037024	33.775757
871.837694	77112.530370	33.780775
872.575473	77219.825827	33.785792
873.674991	77339.226300	33.790810
874.577359	77466.018282	33.795828
876.052699	77574.973163	33.800845
877.074610	77696.148205	33.805863
878.224181	77800.619804	33.810880
879.571167	77898.068032	33.815898
880.332438	78001.435720	33.820916
881.229707	78090.340630	33.825933
881.908290	78196.585035	33.830951
882.613358	78300.596065	33.835968
883.654068	78398.436070	33.840986
884.566087	78512.474242	33.846004
885.497094	78612.194452	33.851021
885.959765	78717.347170	33.856039
886.822173	78822.285672	33.861056
887.569028	78929.611710	33.866074
888.400847	79047.161203	33.871092
889.231005	79159.441235	33.876109
889.735193	79255.962047	33.881127
890.222966	79360.378480	33.886144
891.458341	79465.818448	33.891162
892.319253	79575.954299	33.896180
893.284068	79670.909486	33.901197
894.124548	79797.417801	33.906215
894.759883	79894.807130	33.911232
895.978033	80012.401565	33.916250
896.628768	80120.710109	33.921268
897.094860	80235.420633	33.926285
897.767454	80355.914519	33.931303
898.795551	80480.014713	33.936320
899.631398	80610.252236	33.941338
900.058087	80740.579770	33.946356
900.836819	80862.946973	33.951373
901.466959	81002.163240	33.956391
902.386409	81147.530376	33.961408
903.715028	81277.339082	33.966426
904.284484	81414.970504	33.971444
904.942704	81563.839551	33.976461
905.880338	81710.714460	33.981479
906.778077	81853.111195	33.986496
907.714659	81999.100867	33.991514
908.501742	82138.374184	33.996532
909.653442	82281.556868	34.001549
910.761614	82439.571307	34.006567
911.712170	82581.304576	34.011584
913.165504	82715.091511	34.016602
913.848045	82864.407044	34.021620
914.892634	83002.579959	34.026637
915.698834	83140.664165	34.031655
916.737984	83275.975704	34.036672
917.877487	83410.119137	34.041690
918.836800	83544.734890	34.046708
919.778016	83695.775503	34.051725
920.793738	83823.376765	34.056743
922.341937	83957.218022	34.061760
923.639736	84082.736250	34.066778
924.767894	84205.253206	34.071796
925.651208	84321.650863	34.076813
926.832880	84440.802600	34.081831
927.315967	84573.292962	34.086848
928.714630	84688.090862	34.091866
929.729155	84801.846962	34.096884
930.865658	84926.241034	34.101901
931.440856	85037.089077	34.106919
932.213752	85161.946581	34.111936
933.390608	85280.063477	34.116954
933.992163	85404.872828	34.121972
935.336746	85527.728986	34.126989
936.291862	85652.864192	34.132007
936.831047	85774.707051	34.137024
937.654098	85896.924142	34.142042
938.234186	86029.000473	34.147060
939.157972	86160.060522	34.152077
940.147503	86290.806739	34.157095
940.700364	86423.598749	34.162112
941.933045	86557.476094	34.167130
942.144891	86691.513892	34.172148
943.446454	86826.991047	34.177165
943.996076	86963.701723	34.182183
945.149501	87097.011021	34.187200
945.988193	87246.083950	34.192218
946.975768	87376.087647	34.197236
948.095461	87515.829052	34.202253
949.281635	87651.644891	34.207271
950.341212	87792.943074	34.212288
951.344850	87917.966310	34.217306
952.308645	88047.419094	34.222324
952.896896	88171.013058	34.227341
953.873017	88297.765706	34.232359
954.871155	88433.399143	34.237376
956.022583	88553.206039	34.242394
956.907710	88680.050607	34.247412
957.507917	88811.591336	34.252429
958.468367	88947.372425	34.257447
959.621666	89072.085613	34.262464
960.930488	89189.855400	34.267482
961.688535	89325.745944	34.272500
962.887282	89446.917744	34.277517
963.919602	89587.835865	34.282535
964.315475	89709.159783	34.287552
965.405517	89845.621707	34.292570
966.244441	89985.824247	34.297588
967.763333	90123.994588	34.302605
968.264085	90266.127079	34.307623
969.256335	90406.383617	34.312640
970.353496	90543.722086	34.317658
971.114449	90682.913508	34.322676
971.699956	90820.726240	34.327693
972.575127	90958.177397	34.332711
973.676391	91119.180129	34.337728
974.570824	91252.966818	34.342746
975.407615	91411.287586	34.347764
976.134481	91561.920471	34.352781
977.559835	91717.425728	34.357799
978.303700	91869.781179	34.362816
979.635234	92017.672712	34.367834
980.600226	92166.547589	34.372852
981.395100	92311.546076	34.377869
983.117426	92468.960551	34.382887
983.799661	92616.436991	34.387904
984.709192	92757.122935	34.392922
985.606834	92912.995756	34.397940
986.972419	93059.568825	34.402957
987.985519	93213.828069	34.407975
989.231722	93359.166445	34.412992
990.371686	93495.890461	34.418010
991.309244	93651.570652	34.423028
992.346756	93798.781664	34.428045
993.379653	93935.017385	34.433063
994.586617	94078.894977	34.438080
996.040561	94207.625605	34.443098
996.814973	94348.517428	34.448116
997.877506	94482.748213	34.453133
999.380681	94616.314841	34.458151
1000.317940	94760.212472	34.463168
1001.192157	94875.334400	34.468186
1002.288631	95004.973569	34.473204
1003.599468	95138.255663	34.478221
1004.450273	95264.524619	34.483239
1005.061961	95406.562174	34.488256
1006.472053	95531.958745	34.493274
1007.405984	95672.692146	34.498292
1008.092989	95805.656455	34.503309
1009.252490	95936.671300	34.508327
1010.398656	96071.567654	34.513344
1011.838455	96184.957963	34.518362
1012.661151	96306.431276	34.523380
1013.459438	96443.171029	34.528397
1014.735592	96567.680023	34.533415
1015.382120	96702.923511	34.538432
1016.159624	96836.080825	34.543450
1017.418278	96963.788565	34.548468
1018.118530	97098.733777	34.553485
1019.078880	97231.927511	34.558503
1019.824513	97368.197800	34.563520
1020.725950	97492.312745	34.568538
1021.606081	97623.771308	34.573556
1022.306925	97764.449115	34.578573
1023.098786	97895.200045	34.583591
1023.747065	98058.845051	34.588608
1024.591336	98199.236106	34.593626
1025.518257	98347.728095	34.598644
1025.981534	98494.163624	34.603661
1026.822896	98658.466025	34.608679
1027.853401	98836.456337	34.613696
1029.121132	98992.212672	34.618714
1030.118013	99154.008523	34.623732
1031.173133	99324.974469	34.628749
1032.333145	99482.372742	34.633767
1033.135467	99659.845524	34.638784
1034.277576	99824.246236	34.643802
1035.423887	99989.724722	34.648820
1036.619212	100160.026574	34.653837
1037.839623	100323.631543	34.658855
1038.699222	100498.475654	34.663872
1040.106967	100656.626866	34.668890
1041.224612	100825.296240	34.673908
1042.058181	100990.702003	34.678925
1043.629519	101158.211756	34.683943
1044.611231	101320.388442	34.688960
1045.306966	101482.230359	34.693978
1046.634530	101653.254634	34.698996
1047.244193	101829.336744	34.704013
1048.437354	101990.786326	34.709031
1049.488612	102158.509393	34.714048
1051.087785	102330.293404	34.719066
1052.086153	102501.411657	34.724084
1052.898074	102676.655190	34.729101
1054.314107	102842.980682	34.734119
1055.350603	103002.000060	34.739136
1056.297617	103172.597309	34.744154
1057.296458	103334.654416	34.749172
1058.550446	103518.746446	34.754189
1059.453108	103678.246450	34.759207
1060.254004	103860.547483	34.764224
1061.462646	104029.079492	34.769242
1062.637191	104202.993680	34.774260
1063.589864	104386.884075	34.779277
1064.563869	104549.635636	34.784295
1065.527466	104737.089135	34.789312
1066.781657	104911.425616	34.794330
1067.881582	105085.749112	34.799348
1069.317523	105255.532312	34.804365
1069.962849	105432.756325	34.809383
1070.846547	105606.203415	34.814400
1072.162729	105781.866048	34.819418
1073.502664	105956.524158	34.824436
1074.316907	106144.110261	34.829453
1075.430917	106323.928329	34.834471
1076.597068	106497.602016	34.839488
1078.076669	106665.851128	34.844506
1079.088393	106833.806591	34.849524
1080.081629	107008.625799	34.854541
1081.732982	107174.289100	34.859559
1082.917119	107338.758307	34.864576
1083.785424	107501.806813	34.869594
1085.013260	107681.766336	34.874612
1085.753766	107842.630048	34.879629
1087.400804	108012.723575	34.884647
1088.356075	108169.738308	34.889664
1089.665055	108332.949990	34.894682
1090.588895	108492.164874	34.899700
1091.442206	108650.846250	34.904717
1092.641763	108797.084870	34.909735
1093.214554	108956.864073	34.914752
1094.328225	109101.443523	34.919770
1095.544575	109255.454911	34.924788
1096.422001	109420.616048	34.929805
1097.767962	109582.724522	34.934823
1098.807597	109741.140728	34.939840
1099.538123	109910.892426	34.944858
1100.748976	110069.942734	34.949876
1101.481701	110237.463734	34.954893
1102.712015	110410.132408	34.959911
1103.661254	110591.000182	34.964928
1104.844615	110758.174100	34.969946
1106.140001	110925.141042	34.974964
1107.101300	111103.447836	34.979981
1108.186247	111273.797345	34.984999
1109.139020	111448.087061	34.990016
1110.483016	111622.925112	34.995034
1111.593931	111793.894451	35.000052
1112.811042	111981.055663	35.005069
1113.886480	112152.412728	35.010087
1115.161552	112338.615568	35.015104
1115.827133	112513.564170	35.020122
1117.808023	112686.735092	35.025140
1118.603912	112872.711335	35.030157
1119.598670	113037.617223	35.035175
1121.020927	113228.709716	35.040192
1122.047541	113403.542687	35.045210
1123.238865	113589.473379	35.050228
1124.087041	113759.174163	35.055245
1125.170601	113948.864955	35.060263
1126.130733	114133.160490	35.065280
1127.582494	114314.856091	35.070298
1128.913063	114495.303273	35.075316
1129.577728	114680.801967	35.080333
1130.782222	114861.587760	35.085351
1132.313206	115042.906752	35.090368
1133.682003	115232.635621	35.095386
1134.607707	115406.669538	35.100404
1135.449194	115597.180410	35.105421
1136.854908	115779.854377	35.110439
1137.556519	115967.294300	35.115456
1138.819125	116162.840892	35.120474
1140.141325	116353.305747	35.125492
1140.639254	116547.756446	35.130509
1142.100423	116736.704828	35.135527
1143.032198	116931.837940	35.140544
1144.043262	117127.695315	35.145562
1145.514763	117320.145759	35.150580
1146.572294	117519.967964	35.155597
1147.880815	117710.784316	35.160615
1149.228538	117902.001385	35.165632
1150.194423	118101.752223	35.170650
1151.918832	118296.527300	35.175668
1152.736091	118483.137176	35.180685
1154.027760	118674.595228	35.185703
1155.010779	118859.506659	35.190720
1156.514644	119048.548695	35.195738
1157.461930	119234.342762	35.200756
1158.694592	119430.646648	35.205773
1159.649939	119623.164179	35.210791
1161.176419	119806.663205	35.215808
1162.013765	119997.108096	35.220826
1163.868296	120179.009990	35.225844
1164.959426	120361.374745	35.230861
1166.122821	120544.325238	35.235879
1167.000246	120728.716717	35.240896
1168.145957	120901.853443	35.245914
1169.248252	121082.608826	35.250932
1170.631207	121256.217390	35.255949
1171.807044	121431.153048	35.260967
1172.904130	121603.425212	35.265984
1173.994686	121785.758660	35.271002
1175.181844	121957.041500	35.276020
1176.348599	122128.670788	35.281037
1177.369288	122307.389539	35.286055
1178.460109	122491.832014	35.291072
1179.375168	122681.174159	35.296090
1180.603473	122861.524732	35.301108
1181.494103	123059.270456	35.306125
1182.577336	123258.940631	35.311143
1184.042051	123452.678506	35.316160
1185.470565	123646.067781	35.321178
1186.638892	123840.094967	35.326196
1187.658169	124026.496708	35.331213
1188.784631	124216.865987	35.336231
1190.073833	124406.893533	35.341248
1191.498397	124592.346412	35.346266
1192.648422	124792.483150	35.351284
1193.892072	124987.544347	35.356301
1194.772603	125183.234219	35.361319
1196.229915	125376.475045	35.366336
1196.928312	125580.314710	35.371354
1198.421896	125778.994310	35.376372
1199.610822	125977.215101	35.381389
1201.019786	126174.641198	35.386407
1202.106420	126381.532330	35.391424
1202.998290	126591.664776	35.396442
1204.667747	126790.118746	35.401460
1205.589423	126994.070028	35.406477
1206.839471	127192.020668	35.411495
1208.293253	127395.104024	35.416512
1209.213565	127599.667478	35.421530
1211.079948	127800.607521	35.426548
1212.133406	128007.651523	35.431565
1213.282325	128213.717363	35.436583
1214.427537	128415.153877	35.441600
1215.389919	128627.810363	35.446618
1216.764050	128833.133483	35.451636
1218.105915	129042.713013	35.456653
1219.010591	129265.734859	35.461671
1219.863526	129472.944330	35.466688
1220.710314	129696.332756	35.471706
1222.068718	129910.367409	35.476724
1223.275918	130139.550857	35.481741
1224.361714	130369.503131	35.486759
1225.711328	130590.406788	35.491776
1226.819143	130821.576092	35.496794
1227.917249	131035.568291	35.501812
1229.263133	131263.987416	35.506829
1230.883164	131492.009556	35.511847
1232.389533	131704.025205	35.516864
1233.638293	131925.611268	35.521882
1235.184391	132144.360429	35.526900
1236.532163	132358.345436	35.531917
1237.393710	132577.368877	35.536935
1238.806311	132790.089662	35.541952
1239.831673	133021.791099	35.546970
1241.326925	133237.241887	35.551988
1242.318192	133454.028823	35.557005
1243.717098	133680.866132	35.562023
1245.208012	133892.564841	35.567040
1245.911961	134121.467301	35.572058
1247.182063	134339.331542	35.577076
1248.447656	134558.047727	35.582093
1249.786129	134771.880877	35.587111
1250.885475	134975.930912	35.592128
1251.647259	135192.165797	35.597146
1252.866051	135403.317829	35.602164
1253.984868	135619.295832	35.607181
1254.968431	135851.208796	35.612199
1256.212748	136067.359624	35.617216
1257.595761	136302.511666	35.622234
1258.909572	136517.993881	35.627252
1260.764391	136740.079968	35.632269
1262.297611	136954.045170	35.637287
1263.608983	137170.596778	35.642304
1264.896396	137394.589508	35.647322
1266.094476	137613.318227	35.652340
1267.148349	137828.390407	35.657357
1268.626444	138055.782816	35.662375
1269.999754	138275.210555	35.667392
1271.113268	138503.309417	35.672410
1272.177831	138729.373896	35.677428
1273.266735	138951.577753	35.682445
1274.840228	139174.392086	35.687463
1276.327416	139406.129762	35.692480
1277.693979	139633.572637	35.697498
1278.880907	139843.328511	35.702516
1280.461287	140070.562333	35.707533
1281.514996	140302.511828	35.712551
1283.407384	140536.526679	35.717568
1284.282403	140760.104998	35.722586
1285.925253	140974.083987	35.727604
1287.417014	141192.986320	35.732621
1288.847021	141415.211688	35.737639
1289.915570	141634.816820	35.742656
1291.462593	141861.747024	35.747674
1292.516308	142075.721560	35.752692
1293.895315	142286.714414	35.757709
1295.099219	142526.075459	35.762727
1297.008556	142735.096204	35.767744
1297.899514	142957.958689	35.772762
1299.020113	143182.588432	35.777780
1300.441882	143405.966344	35.782797
1302.245278	143636.100950	35.787815
1303.778152	143844.576102	35.792832
1304.843935	144066.020093	35.797850
1306.400242	144289.292053	35.802868
1307.185382	144514.906802	35.807885
1307.928245	144730.718296	35.812903
1309.571581	144955.794533	35.817920
1311.032606	145181.839520	35.822938
1312.192025	145406.561975	35.827956
1313.782522	145627.943359	35.832973
1315.239497	145848.369300	35.837991
1316.242918	146075.314869	35.843008
1317.677791	146300.772358	35.848026
1318.749189	146527.963126	35.853044
1319.906938	146762.160302	35.858061
1320.925094	146998.474651	35.863079
1322.262944	147230.170704	35.868096
1323.269899	147462.198819	35.873114
1324.536674	147712.401295	35.878132
1325.872120	147948.530650	35.883149
1326.735287	148201.426027	35.888167
1327.682910	148454.779029	35.893184
1329.165906	148699.672105	35.898202
1330.743855	148955.505491	35.903220
1332.353979	149198.730873	35.908237
1333.700419	149445.743100	35.913255
1335.248181	149692.217223	35.918272
1336.579504	149925.982364	35.923290
1338.141259	150163.482347	35.928308
1339.661444	150379.423921	35.933325
1341.322792	150600.523152	35.938343
1342.648525	150824.442981	35.943360
1343.614004	151058.638365	35.948378
1344.871893	151282.951490	35.953396
1346.152022	151505.040671	35.958413
1347.060067	151748.983957	35.963431
1348.515875	151975.312588	35.968448
1349.600204	152215.815729	35.973466
1350.156447	152461.746658	35.978484
1351.578401	152713.598123	35.983501
1352.798188	152971.994341	35.988519
1354.410037	153225.963647	35.993536
1355.488846	153480.169860	35.998554
1356.771005	153752.231347	36.003572
1358.192866	154001.790932	36.008589
1359.042629	154281.831078	36.013607
1360.312324	154556.462570	36.018624
1362.015710	154821.887570	36.023642
1363.216620	155098.360389	36.028660
1364.971628	155362.319929	36.033677
1366.048575	155641.505954	36.038695
1367.543256	155910.231075	36.043712
1369.082392	156181.451306	36.048730
1370.422870	156457.769057	36.053748
1372.260556	156728.932374	36.058765
1373.914375	157007.514080	36.063783
1375.704050	157277.786080	36.068800
1376.848064	157535.478150	36.073818
1378.735882	157800.049821	36.078836
1380.276888	158060.398716	36.083853
1381.585646	158330.496813	36.088871
1383.142197	158588.255742	36.093888
1384.559076	158848.208496	36.098906
1385.378615	159111.810517	36.103924
1386.841857	159369.600028	36.108941
1388.381275	159641.026184	36.113959
1389.875318	159903.650021	36.118976
1391.090714	160163.614450	36.123994
1392.614614	160438.563146	36.129012
1394.324393	160692.688623	36.134029
1396.006479	160969.900078	36.139047
1397.202019	161232.157234	36.144064
1398.825459	161479.710331	36.149082
1400.219327	161754.037606	36.154100
1402.016333	162004.142804	36.159117
1403.362172	162257.747478	36.164135
1404.922117	162504.793931	36.169152
1406.307429	162766.151621	36.174170
1407.591374	163036.261085	36.179188
1409.229175	163280.289333	36.184205
1410.970048	163537.214303	36.189223
1412.078748	163780.641631	36.194240
1413.951668	164029.625440	36.199258
1415.332528	164290.113834	36.204276
1416.935814	164534.329849	36.209293
1418.457288	164783.104853	36.214311
1420.011063	165031.113936	36.219328
1421.503019	165270.855521	36.224346
1422.668229	165529.020919	36.229364
1423.871956	165755.871602	36.234381
1425.059640	166004.906470	36.239399
1426.349017	166247.616099	36.244416
1427.400352	166504.647596	36.249434
1429.014077	166753.643871	36.254452
1430.305094	167003.047057	36.259469
1431.751633	167257.048428	36.264487
1432.835096	167509.393471	36.269504
1434.187337	167746.359492	36.274522
1435.161983	167999.485129	36.279540
1436.704715	168244.866464	36.284557
1437.879648	168494.140714	36.289575
1439.131143	168748.127156	36.294592
1440.616172	169008.083678	36.299610
1441.564315	169278.930455	36.304628
1443.158962	169528.396518	36.309645
1444.443150	169820.130409	36.314663
1446.036388	170080.657887	36.319680
1447.137526	170340.095152	36.324698
1448.475297	170625.627529	36.329716
1449.776604	170902.608626	36.334733
1451.193562	171197.552297	36.339751
1452.367565	171476.053736	36.344768
1453.513036	171766.788443	36.349786
1455.167024	172071.145421	36.354804
1456.409704	172366.730391	36.359821
1457.685923	172662.527107	36.364839
1458.779345	172966.873778	36.369856
1460.919918	173271.908492	36.374874
1461.973791	173585.533183	36.379892
1463.716421	173877.934645	36.384909
1465.662958	174183.460381	36.389927
1467.524992	174484.238751	36.394944
1469.119512	174788.767958	36.399962
1470.587086	175081.991454	36.404980
1472.121221	175372.361199	36.409997
1473.936914	175679.271778	36.415015
1475.707883	175985.961935	36.420032
1477.250389	176275.635155	36.425050
1478.989009	176570.751678	36.430068
1480.671121	176859.020951	36.435085
1481.886640	177154.957908	36.440103
1483.141340	177455.791383	36.445120
1484.757400	177735.210429	36.450138
1486.313405	178038.157542	36.455156
1487.553766	178331.935924	36.460173
1489.325239	178631.854515	36.465191
1490.637829	178933.471392	36.470208
1492.480698	179229.114086	36.475226
1493.408658	179534.450455	36.480244
1494.825313	179831.152367	36.485261
1495.982004	180140.569425	36.490279
1497.403153	180445.145958	36.495296
1498.931762	180750.925792	36.500314
1500.700248	181056.618306	36.505332
1502.522349	181378.050260	36.510349
1503.912784	181681.619772	36.515367
1505.416144	181995.306501	36.520384
1507.141758	182304.057607	36.525402
1508.720642	182609.962660	36.530420
1510.455106	182916.606297	36.535437
1512.092069	183217.272104	36.540455
1513.024676	183525.186110	36.545472
1514.514505	183825.546641	36.550490
1516.118068	184133.560733	36.555508
1517.892416	184448.152766	36.560525
1519.957876	184749.111771	36.565543
1521.304501	185064.661647	36.570560
1523.329704	185383.230392	36.575578
1524.401421	185734.866753	36.580596
1526.183338	186017.662642	36.585613
1527.680509	186319.096203	36.590631
1529.310551	186615.379149	36.595648
1530.628791	186916.664633	36.600666
1532.403964	187209.624590	36.605684
1533.897596	187482.436692	36.610701
1535.129720	187757.576387	36.615719
1536.768807	188040.222217	36.620736
1538.385123	188309.766023	36.625754
1539.492073	188600.192728	36.630772
1540.680740	188893.299799	36.635789
1542.105753	189187.437446	36.640807
1543.139679	189488.495097	36.645824
1544.665127	189787.597000	36.650842
1545.955878	190094.915290	36.655860
1547.038109	190406.407281	36.660877
1549.139890	190709.612410	36.665895
1550.422230	191028.644041	36.670912
1551.798514	191353.097531	36.675930
1552.928861	191678.454008	36.680948
1554.786974	192000.573174	36.685965
1556.812604	192319.060068	36.690983
1557.972642	192647.665759	36.696000
1559.729382	192962.513272	36.701018
1561.505631	193284.115157	36.706036
1563.073588	193616.317256	36.711053
1564.482537	193940.365964	36.716071
1566.263348	194269.767712	36.721088
1568.069551	194591.139545	36.726106
1569.582544	194930.262696	36.731124
1570.979155	195263.562621	36.736141
1572.313865	195595.984004	36.741159
1573.339085	195937.700741	36.746176
1575.234861	196269.934326	36.751194
1577.034112	196623.521091	36.756212
1578.120243	196972.063818	36.761229
1580.359339	197312.933452	36.766247
1581.788853	197663.888060	36.771264
1583.502599	198007.381698	36.776282
1585.298702	198344.563582	36.781300
1587.097033	198680.348763	36.786317
1588.740931	199016.489075	36.791335
1590.314162	199372.734155	36.796352
1591.741996	199717.292447	36.801370
1592.993797	200058.779976	36.806388
1594.758654	200403.845841	36.811405
1596.790399	200751.588699	36.816423
1598.110853	201113.364050	36.821440
1599.732423	201453.374062	36.826458
1601.285061	201811.304211	36.831476
1602.936513	202164.113743	36.836493
1604.831976	202519.629260	36.841511
1605.728883	202879.721800	36.846528
1607.648218	203229.417798	36.851546
1609.091944	203586.073003	36.856564
1610.574594	203938.277325	36.861581
1612.926123	204293.343833	36.866599
1614.139620	204653.059982	36.871616
1616.110459	205010.854660	36.876634
1617.705468	205366.346326	36.881652
1619.281196	205719.428352	36.886669
1621.188728	206078.784379	36.891687
1622.274101	206432.884251	36.896704
1624.047383	206801.839424	36.901722
1625.487200	207149.762857	36.906740
1626.594548	207518.671018	36.911757
1628.690010	207873.961462	36.916775
1630.521913	208234.145700	36.921792
1632.721619	208584.340259	36.926810
1634.011845	208933.331283	36.931828
1635.675033	209287.903956	36.936845
1637.526638	209645.521437	36.941863
1639.129005	210002.238489	36.946880
1640.709360	210347.324709	36.951898
1642.081328	210681.444293	36.956916
1643.466981	211021.023879	36.961933
1645.302370	211358.577415	36.966951
1646.666337	211694.960345	36.971968
1648.338943	212040.008765	36.976986
1650.050544	212393.002787	36.982004
1651.121999	212743.379199	36.987021
1652.890283	213094.002586	36.992039
1654.209166	213454.197637	36.997056
1656.057591	213810.804483	37.002074
1657.612882	214164.891788	37.007092
1658.750081	214536.268594	37.012109
1660.826822	214909.048354	37.017127
1662.608520	215293.484167	37.022144
1663.962005	215658.019970	37.027162
1665.449618	216031.909106	37.032180
1666.794261	216405.973356	37.037197
1668.803984	216791.238545	37.042215
1670.447921	217172.471264	37.047232
1672.088738	217552.637796	37.052250
1673.557586	217950.817489	37.057268
1674.999096	218341.964855	37.062285
1676.810186	218729.218646	37.067303
1678.446183	219139.439864	37.072320
1680.005240	219542.966725	37.077338
1681.991291	219941.778060	37.082356
1683.401527	220356.760455	37.087373
1685.453035	220746.924587	37.092391
1687.175830	221155.126387	37.097408
1689.300114	221550.512695	37.102426
1691.323305	221945.635522	37.107444
1693.457049	222341.630318	37.112461
1695.292603	222736.046032	37.117479
1697.042640	223123.641531	37.122496
1699.086840	223506.719958	37.127514
1700.521189	223893.196418	37.132532
1702.606581	224279.901297	37.137549
1704.819553	224652.004303	37.142567
1706.646973	225037.885874	37.147584
1708.263610	225417.449419	37.152602
1710.019699	225786.727886	37.157620
1711.473295	226180.670232	37.162637
1713.643474	226541.856159	37.167655
1715.652989	226926.464345	37.172672
1716.966344	227303.458578	37.177690
1718.810025	227670.030292	37.182708
1720.479504	228055.123348	37.187725
1722.482963	228430.408880	37.192743
1724.300967	228821.677070	37.197760
1725.854198	229191.062875	37.202778
1727.564623	229566.089050	37.207796
1728.823425	229941.820853	37.212813
1730.485610	230318.810378	37.217831
1732.248888	230702.668391	37.222848
1734.032215	231081.010406	37.227866
1736.083850	231473.409435	37.232884
1737.693730	231854.521793	37.237901
1739.434597	232224.181649	37.242919
1741.146238	232606.547806	37.247936
1742.809992	232979.343924	37.252954
1744.754893	233362.130319	37.257972
1746.217303	233751.139664	37.262989
1748.331419	234138.928941	37.268007
1749.806488	234522.981920	37.273024
1751.176368	234900.192000	37.278042
1752.950900	235290.904039	37.283060
1754.505730	235681.370644	37.288077
1755.825682	236057.012437	37.293095
1757.335972	236442.023441	37.298112
1758.867174	236816.767685	37.303130
1760.490741	237196.857247	37.308148
1761.773392	237596.662138	37.313165
1763.499949	237988.521969	37.318183
1765.006957	238388.875064	37.323200
1766.777940	238794.317847	37.328218
1768.497091	239194.179431	37.333236
1769.683223	239610.051844	37.338253
1771.796083	240020.367704	37.343271
1773.437226	240445.465328	37.348288
1775.065299	240873.409500	37.353306
1776.737655	241295.757319	37.358324
1778.099002	241731.083362	37.363341
1779.974495	242157.157629	37.368359
1781.806786	242605.313250	37.373376
1783.632312	243051.487636	37.378394
1785.395303	243486.264970	37.383412
1786.692457	243932.621920	37.388429
1788.900417	244377.362063	37.393447
1790.658334	244827.150675	37.398464
1792.060150	245290.635371	37.403482
1794.516412	245741.328827	37.408500
1796.235101	246201.434082	37.413517
1798.091070	246652.270201	37.418535
1800.139541	247119.485217	37.423552
1801.547237	247585.198978	37.428570
1803.591923	248035.443377	37.433588
1804.975047	248492.471006	37.438605
1807.587451	248958.297518	37.443623
1809.246998	249428.945897	37.448640
1811.005279	249897.875569	37.453658
1813.011119	250351.295278	37.458676
1815.244112	250824.415583	37.463693
1817.439422	251274.881813	37.468711
1819.486936	251736.699133	37.473728
1821.253103	252196.552353	37.478746
1823.243661	252641.458234	37.483764
1824.942233	253109.549412	37.488781
1826.488618	253570.093236	37.493799
1828.742388	254026.206641	37.498816
1830.146760	254496.904914	37.503834
1832.175710	254951.221603	37.508852
1834.115987	255416.142997	37.513869
1835.635506	255880.900026	37.518887
1837.525406	256347.705771	37.523904
1839.418351	256809.327579	37.528922
1841.663899	257279.198663	37.533940
1843.703682	257737.619049	37.538957
1845.422997	258195.757702	37.543975
1847.330246	258663.517494	37.548992
1848.760752	259123.323532	37.554010
1851.155294	259588.438060	37.559028
1852.609951	260057.050686	37.564045
1854.186115	260528.563456	37.569063
1856.573476	260989.609523	37.574080
1858.505672	261463.907565	37.579098
1860.119974	261922.784811	37.584116
1861.964679	262390.641048	37.589133
1863.797875	262857.785905	37.594151
1865.665010	263329.266774	37.599168
1867.769269	263803.223017	37.604186
1869.650148	264261.997875	37.609204
1871.312864	264736.628596	37.614221
1873.065597	265202.404157	37.619239
1874.901990	265679.822656	37.624256
1876.503305	266142.950707	37.629274
1878.765043	266601.299896	37.634292
1880.668651	267054.191487	37.639309
1882.261523	267497.579749	37.644327
1884.363279	267950.156779	37.649344
1886.147506	268414.159796	37.654362
1888.004488	268857.602024	37.659380
1890.167076	269312.271075	37.664397
1891.775711	269762.783121	37.669415
1893.884045	270209.786061	37.674432
1895.331080	270669.766906	37.679450
1897.151474	271131.693386	37.684468
1898.917852	271591.035386	37.689485
1900.902010	272059.204570	37.694503
1902.978297	272532.055300	37.699520
1904.785618	273014.672583	37.704538
1906.555453	273477.635835	37.709556
1908.264012	273962.904471	37.714573
1910.346043	274441.305579	37.719591
1912.175840	274923.222710	37.724608
1913.794965	275415.430079	37.729626
1916.091740	275896.760484	37.734644
1917.667057	276378.531052	37.739661
1919.781444	276874.588399	37.744679
1922.328646	277354.093132	37.749696
1923.814662	277856.362972	37.754714
1925.423989	278344.617440	37.759732
1927.480253	278841.255471	37.764749
1929.347689	279345.106599	37.769767
1931.689237	279836.741449	37.774784
1933.780000	280344.512529	37.779802
1935.581913	280839.044007	37.784820
1937.669556	281339.749059	37.789837
1940.004571	281846.836680	37.794855
1941.878282	282344.038483	37.799872
1943.810766	282855.600519	37.804890
1945.587992	283359.514288	37.809908
1947.710913	283854.330297	37.814925
1949.310251	284368.218860	37.819943
1951.543750	284878.474741	37.824960
1952.967063	285387.787089	37.829978
1955.133706	285898.248945	37.834996
1956.893052	286427.357948	37.840013
1958.756932	286935.954841	37.845031
1960.652279	287450.408472	37.850048
1962.898682	287973.639517	37.855066
1964.960046	288492.984991	37.860084
1967.409377	289007.847469	37.865101
1969.194464	289530.274769	37.870119
1971.603954	290039.320556	37.875136
1973.473373	290555.327652	37.880154
1975.624603	291066.436784	37.885172
1977.723079	291578.464015	37.890189
1979.923966	292082.473045	37.895207
1982.115742	292590.490963	37.900224
1984.127847	293102.011137	37.905242
1986.119121	293615.891452	37.910260
1988.181874	294109.241559	37.915277
1990.127286	294616.341449	37.920295
1992.470046	295103.749156	37.925312
1994.563706	295600.306323	37.930330
1996.954099	296108.034528	37.935348
1999.009029	296599.993850	37.940365
2000.686652	297096.704766	37.945383
2003.208393	297581.499311	37.950400
2004.991126	298065.288262	37.955418
2006.704025	298559.035824	37.960436
2008.579446	299051.712705	37.965453
2010.600918	299543.397642	37.970471
2012.884808	300018.916552	37.975488
2014.399849	300490.743638	37.980506
2016.444620	300952.836950	37.985524
2018.622832	301425.339095	37.990541
2020.067525	301894.372436	37.995559
2022.200651	302369.767265	38.000576
2024.031201	302863.863420	38.005594
2025.714406	303345.158488	38.010612
2027.872704	303825.283239	38.015629
2029.132132	304327.628851	38.020647
2031.445494	304829.474678	38.025664
2033.192425	305333.130338	38.030682
2034.764982	305826.553201	38.035700
2036.809986	306354.419119	38.040717
2038.541453	306873.545901	38.045735
2040.581016	307394.649738	38.050752
2042.625424	307922.118447	38.055770
2044.493834	308445.192484	38.060788
2046.908368	308980.866653	38.065805
2048.388552	309519.143173	38.070823
2051.025856	310053.653844	38.075840
2053.232427	310603.124881	38.080858
2055.496843	311136.894989	38.085876
2057.382067	311677.241311	38.090893
2059.140129	312233.591113	38.095911
2061.176108	312768.850575	38.100928
2063.218037	313316.488397	38.105946
2064.782402	313879.650690	38.110964
2066.809586	314439.129812	38.115981
2069.183830	315005.831579	38.120999
2070.887923	315566.108789	38.126016
2072.867838	316142.831870	38.131034
2075.162452	316728.786682	38.136052
2077.408425	317306.087588	38.141069
2079.500170	317869.142983	38.146087
2081.554364	318440.292349	38.151104
2083.693369	319019.262413	38.156122
2085.943254	319599.349359	38.161140
2088.051893	320178.156436	38.166157
2090.239926	320764.809771	38.171175
2092.537502	321339.257716	38.176192
2094.674735	321928.541997	38.181210
2096.904968	322514.910777	38.186228
2099.194303	323093.472186	38.191245
2100.904519	323688.431634	38.196263
2103.272411	324260.138902	38.201280
2105.531796	324839.923904	38.206298
2107.900263	325423.159715	38.211316
2110.403605	325996.343908	38.216333
2112.617776	326578.902183	38.221351
2115.334714	327143.486231	38.226368
2117.142039	327719.824745	38.231386
2119.406335	328286.264803	38.236404
2121.919050	328841.038086	38.241421
2124.375757	329402.307122	38.246439
2126.920023	329952.543819	38.251456
2129.450415	330502.039186	38.256474
2131.639051	331047.013745	38.261492
2134.009133	331586.624726	38.266509
2135.641682	332139.864946	38.271527
2137.627555	332676.349576	38.276544
2140.164880	333230.903724	38.281562
2142.161065	333768.944049	38.286580
2144.092364	334328.168353	38.291597
2145.546682	334875.384342	38.296615
2147.423247	335418.645163	38.301632
2149.923285	335987.470831	38.306650
2152.009634	336536.288243	38.311668
2154.143833	337059.141321	38.316685
2156.471473	337601.157826	38.321703
2158.464407	338125.311268	38.326720
2160.606413	338654.354412	38.331738
2162.353725	339187.230705	38.336756
2164.597556	339711.397834	38.341773
2166.264690	340254.948687	38.346791
2168.274239	340788.089693	38.351808
2170.107480	341329.340759	38.356826
2172.397220	341875.305436	38.361844
2174.627610	342446.530811	38.366861
2176.309246	343004.568852	38.371879
2178.385610	343571.412332	38.376896
2180.510131	344136.362289	38.381914
2182.427466	344707.091995	38.386932
2184.610136	345296.967615	38.391949
2186.600553	345879.204679	38.396967
2188.988641	346463.550306	38.401984
2191.367666	347049.636881	38.407002
2193.180973	347648.581863	38.412020
2195.693594	348245.530234	38.417037
2197.689228	348835.778502	38.422055
2200.086344	349447.404670	38.427072
2201.895697	350047.523836	38.432090
2203.926116	350662.734421	38.437108
2206.284560	351273.952046	38.442125
2208.122952	351894.062725	38.447143
2210.241863	352511.683594	38.452160
2212.505154	353138.473168	38.457178
2214.745754	353778.665531	38.462196
2217.002369	354399.878986	38.467213
2219.388226	355039.769532	38.472231
2221.437086	355678.280067	38.477248
2223.603318	356297.720812	38.482266
2226.041769	356946.056494	38.487284
2228.262735	357580.850539	38.492301
2230.756304	358225.601720	38.497319
2233.100904	358877.384162	38.502336
2235.806290	359516.929156	38.507354
2237.556528	360152.934679	38.512372
2240.456769	360791.763165	38.517389
2242.385036	361434.684137	38.522407
2244.442810	362099.241706	38.527424
2246.919831	362735.129345	38.532442
2249.456451	363379.205681	38.537460
2251.926288	364026.142260	38.542477
2254.308547	364663.827826	38.547495
2256.391104	365293.842032	38.552512
2258.969668	365945.255427	38.557530
2261.094098	366587.779467	38.562548
2263.430308	367223.413847	38.567565
2265.642735	367871.951951	38.572583
2267.546326	368521.511876	38.577600
2270.147031	369167.096245	38.582618
2272.267256	369826.981569	38.587636
2274.708548	370456.318984	38.592653
2276.986439	371118.885798	38.597671
2279.520094	371760.265533	38.602688
2281.857783	372406.449725	38.607706
2283.683718	373067.039087	38.612724
2285.980936	373701.595284	38.617741
2288.446142	374357.999858	38.622759
2290.739838	375007.524511	38.627776
2293.088971	375662.319677	38.632794
2295.439384	376309.422837	38.637812
2297.241619	376956.216186	38.642829
2299.844561	377610.366881	38.647847
2301.884364	378265.526865	38.652864
2304.082348	378887.665459	38.657882
2306.377465	379538.245160	38.662900
2308.936198	380157.207103	38.667917
2311.070072	380781.261319	38.672935
2313.156082	381412.729263	38.677952
2315.835167	382051.104829	38.682970
2318.014817	382682.552536	38.687988
2319.953034	383312.604269	38.693005
2322.230803	383959.327716	38.698023
2324.296757	384611.259575	38.703040
2327.055821	385247.719729	38.708058
2329.037586	385900.062207	38.713076
2331.331092	386553.681196	38.718093
2333.709098	387218.589112	38.723111
2335.621606	387866.637249	38.728128
2338.089573	388536.307177	38.733146
2340.518903	389212.269877	38.738164
2342.734437	389884.373631	38.743181
2345.160647	390558.046511	38.748199
2347.406211	391230.007502	38.753216
2349.441410	391910.287102	38.758234
2351.746450	392608.126042	38.763252
2354.025632	393304.885647	38.768269
2356.561758	394000.825474	38.773287
2358.537027	394701.541408	38.778304
2360.960015	395396.850854	38.783322
2363.321459	396113.058345	38.788340
2365.926861	396812.854215	38.793357
2367.784428	397538.614878	38.798375
2370.233700	398263.956865	38.803392
2372.855815	398979.074688	38.808410
2374.853855	399697.912751	38.813428
2377.765539	400423.368343	38.818445
2380.512871	401159.557368	38.823463
2382.873124	401881.307840	38.828480
2385.058886	402600.228606	38.833498
2387.686045	403323.055944	38.838516
2390.119821	404048.775276	38.843533
2393.066824	404769.988229	38.848551
2395.382390	405498.260495	38.853568
2397.888528	406220.761071	38.858586
2400.037878	406947.898958	38.863604
2402.764057	407669.913402	38.868621
2405.407706	408390.652282	38.873639
2407.859057	409122.478612	38.878656
2410.492362	409838.061460	38.883674
2412.525331	410582.452392	38.888692
2415.146341	411297.635273	38.893709
2417.910993	412022.940934	38.898727
2420.555738	412748.898727	38.903744
2423.078332	413464.379596	38.908762
2425.912107	414198.201200	38.913780
2428.407921	414924.058237	38.918797
2430.382068	415642.637732	38.923815
2432.797147	416363.652988	38.928832
2435.461651	417075.702780	38.933850
2437.652895	417804.998788	38.938868
2440.460615	418518.595817	38.943885
2443.026217	419233.622440	38.948903
2445.306724	419956.254921	38.953920
2447.979643	420673.541575	38.958938
2449.978274	421379.176944	38.963956
2452.715550	422100.550572	38.968973
2455.532339	422813.846592	38.973991
2457.550151	423525.523564	38.979008
2460.304309	424233.318970	38.984026
2462.814250	424946.689465	38.989044
2464.896173	425656.916612	38.994061
2467.829833	426347.571972	38.999079
2469.705629	427032.302522	39.004096
2472.199372	427708.116832	39.009114
2474.269304	428402.678396	39.014132
2476.646681	429095.448938	39.019149
2479.082562	429782.272058	39.024167
2481.021948	430487.497011	39.029184
2483.579880	431183.552600	39.034202
2486.163068	431902.879385	39.039220
2488.271766	432613.914784	39.044237
2490.527846	433332.886210	39.049255
2492.468966	434065.272393	39.054272
2495.158219	434787.811202	39.059290
2497.850220	435524.016792	39.064308
2500.547398	436253.422231	39.069325
2502.749767	436983.887816	39.074343
2505.262153	437732.668632	39.079360
2508.098802	438473.032628	39.084378
2510.363400	439228.411845	39.089396
2512.698514	439975.514899	39.094413
2515.262827	440730.887970	39.099431
2517.734323	441488.972969	39.104448
2520.434629	442256.993241	39.109466
2523.168278	443023.461179	39.114484
2525.430665	443796.688969	39.119501
2528.145743	444551.024489	39.124519
2530.250269	445331.334195	39.129536
2533.065591	446104.782460	39.134554
2535.475309	446896.745039	39.139572
2537.797182	447687.525375	39.144589
2540.359179	448466.518247	39.149607
2542.994138	449267.078027	39.154624
2545.864496	450071.402812	39.159642
2548.155128	450862.503125	39.164660
2550.679381	451649.644240	39.169677
2553.640651	452457.179556	39.174695
2556.109847	453266.118104	39.179712
2559.068884	454051.418585	39.184730
2561.841158	454851.200787	39.189748
2564.633409	455652.760553	39.194765
2567.637566	456434.868123	39.199783
2569.988394	457223.301318	39.204800
2572.460058	458013.042481	39.209818
2575.754292	458807.817099	39.214836
2578.045866	459597.867180	39.219853
2580.667541	460385.407046	39.224871
2583.680913	461184.354463	39.229888
2586.116421	461967.864070	39.234906
2589.187134	462760.774408	39.239924
2590.849492	463549.831581	39.244941
2593.792927	464342.384907	39.249959
2596.110187	465143.171550	39.254976
2598.590735	465930.677386	39.259994
2601.264649	466736.729761	39.265012
2604.085942	467538.785593	39.270029
2606.682256	468338.820255	39.275047
2609.125110	469147.364027	39.280064
2611.774029	469949.077685	39.285082
2614.193709	470755.528648	39.290100
2616.663722	471561.175553	39.295117
2619.778471	472368.648469	39.300135
2622.335175	473176.370236	39.305152
2624.603674	473978.298283	39.310170
2627.313313	474790.100540	39.315188
2630.079145	475597.214698	39.320205
2632.970031	476398.168538	39.325223
2635.197718	477209.117076	39.330240
2638.024548	478000.371854	39.335258
2640.619431	478780.029918	39.340276
2643.551554	479565.695745	39.345293
2646.231077	480332.461279	39.350311
2648.482203	481108.177107	39.355328
2651.444854	481871.244857	39.360346
2653.919594	482646.849457	39.365364
2656.679158	483428.317136	39.370381
2659.385424	484197.559612	39.375399
2661.802358	484983.991014	39.380416
2664.445324	485760.219768	39.385434
2666.846906	486543.651691	39.390452
2669.314813	487333.380991	39.395469
2672.224071	488139.725452	39.400487
2674.758885	488939.889841	39.405504
2677.218493	489740.376448	39.410522
2679.808230	490538.483450	39.415540
2682.566391	491351.379818	39.420557
2685.272693	492154.369235	39.425575
2687.530149	492985.335833	39.430592
2690.140205	493805.626052	39.435610
2692.578357	494640.803003	39.440628
2694.888943	495493.324333	39.445645
2697.686355	496334.996148	39.450663
2700.366070	497190.785606	39.455680
2702.905343	498041.059861	39.460698
2705.752630	498903.922361	39.465716
2708.321781	499767.532481	39.470733
2711.024461	500635.902607	39.475751
2713.877086	501507.468877	39.480768
2716.490503	502368.753147	39.485786
2719.251853	503247.677283	39.490804
2721.841280	504137.142187	39.495821
2724.798434	505034.444747	39.500839
2727.167704	505919.858076	39.505856
2730.130518	506802.557582	39.510874
2733.118705	507706.680291	39.515892
2735.583373	508596.037075	39.520909
2738.520241	509491.853588	39.525927
2741.358062	510406.993847	39.530944
2743.986598	511304.905660	39.535962
2747.171551	512206.746435	39.540980
2749.291155	513125.844186	39.545997
2752.495266	514026.909982	39.551015
2755.237529	514933.922667	39.556032
2758.056706	515851.321816	39.561050
2761.046509	516758.426831	39.566068
2764.216611	517666.298151	39.571085
2767.400874	518564.203640	39.576103
2770.426426	519469.614621	39.581120
2773.132118	520372.200380	39.586138
2776.364486	521267.154739	39.591156
2779.157911	522161.213625	39.596173
2782.390053	523038.611031	39.601191
2785.443091	523926.933384	39.606208
2788.419576	524809.530673	39.611226
2791.500333	525686.928253	39.616244
2793.926048	526569.092739	39.621261
2796.929842	527444.275764	39.626279
2799.814097	528324.995225	39.631296
2802.200078	529211.309058	39.636314
2805.012556	530082.026457	39.641332
2807.545394	530970.106698	39.646349
2810.834704	531841.084013	39.651367
2813.566772	532722.635416	39.656384
2816.356688	533601.506628	39.661402
2819.354810	534485.356539	39.666420
2821.712596	535360.007924	39.671437
2824.753455	536230.677424	39.676455
2827.437772	537087.438188	39.681472
2830.182226	537931.733570	39.686490
2833.204409	538770.558820	39.691508
2835.663678	539613.783029	39.696525
2838.317748	540450.597087	39.701543
2840.724422	541314.894278	39.706560
2843.437421	542161.722168	39.711578
2845.904770	543031.662201	39.716596
2848.424935	543907.253016	39.721613
2851.067355	544780.806595	39.726631
2853.890397	545662.447383	39.731648
2856.612730	546555.327462	39.736666
2859.348721	547435.751873	39.741684
2862.083225	548350.519282	39.746701
2864.883307	549251.517223	39.751719
2867.592264	550153.265427	39.756736
2870.608131	551066.883160	39.761754
2873.622271	551991.011903	39.766772
2876.241673	552917.488320	39.771789
2879.015674	553845.924973	39.776807
2881.727315	554774.049248	39.781824
2884.583313	555727.241345	39.786842
2887.863844	556664.804281	39.791860
2890.856956	557613.364030	39.796877
2893.349095	558564.632607	39.801895
2896.245332	559526.384614	39.806912
2898.893793	560483.237196	39.811930
2902.149145	561444.776957	39.816948
2905.321568	562415.869407	39.821965
2908.601352	563367.028560	39.826983
2911.444808	564343.622828	39.832000
2914.494903	565319.852574	39.837018
2917.226887	566282.328517	39.842036
2919.837068	567264.272628	39.847053
2922.781383	568241.174161	39.852071
2926.049809	569220.946114	39.857088
2928.418663	570212.139124	39.862106
2931.574840	571198.467885	39.867124
2935.009322	572195.879741	39.872141
2937.905253	573188.383606	39.877159
2941.080632	574179.255606	39.882176
2943.165720	575163.005537	39.887194
2946.717462	576155.846972	39.892212
2949.618580	577168.814871	39.897229
2952.211962	578175.836210	39.902247
2954.999723	579184.487154	39.907264
2957.976957	580208.072333	39.912282
2961.309704	581230.957416	39.917300
2963.879850	582248.316316	39.922317
2966.585716	583263.810086	39.927335
2969.944265	584285.857903	39.932352
2972.585017	585310.072453	39.937370
2975.727192	586336.512155	39.942388
2978.603083	587373.143696	39.947405
2981.393607	588409.339840	39.952423
2984.702325	589444.706174	39.957440
2987.444796	590498.101052	39.962458
2990.288372	591531.091120	39.967476
2993.483876	592573.269381	39.972493
2996.284817	593618.704909	39.977511
2999.205502	594670.812576	39.982528
3002.262006	595721.796011	39.987546
3005.680373	596771.719749	39.992564
3008.462733	597823.436330	39.997581
3011.311196	598869.994596	40.002599
3014.132212	599914.156313	40.007616
3016.865084	600976.448868	40.012634
3020.026991	602024.240434	40.017652
3023.139644	603053.267572	40.022669
3026.312745	604078.041043	40.027687
3029.281873	605095.209871	40.032704
3032.387916	606119.541866	40.037722
3035.058631	607125.879119	40.042740
3038.260683	608146.252190	40.047757
3041.657390	609174.873096	40.052775
3044.379738	610186.088891	40.057792
3046.907443	611225.760959	40.062810
3050.177833	612252.544336	40.067828
3053.585235	613291.567561	40.072845
3056.468321	614330.465972	40.077863
3059.708036	615367.655893	40.082880
3062.640554	616407.926792	40.087898
3065.747837	617442.330456	40.092916
3069.068209	618504.700452	40.097933
3072.149084	619553.889080	40.102951
3075.205300	620596.842044	40.107968
3078.556612	621657.723146	40.112986
3081.787809	622723.241078	40.118004
3084.782909	623784.396804	40.123021
3087.663562	624846.650716	40.128039
3090.958038	625905.138945	40.133056
3094.126900	626980.112513	40.138074
3096.936484	628051.737306	40.143092
3100.445516	629119.052055	40.148109
3104.043769	630203.805573	40.153127
3107.444044	631262.736694	40.158144
3110.591269	632336.370556	40.163162
3113.526227	633424.894529	40.168180
3116.254564	634506.560188	40.173197
3119.485365	635594.342219	40.178215
3122.856019	636666.159741	40.183232
3126.403119	637754.987146	40.188250
3129.505252	638832.519326	40.193268
3132.911978	639913.510295	40.198285
3135.610034	640993.741636	40.203303
3139.471435	642075.754228	40.208320
3142.295268	643166.551923	40.213338
3145.775536	644235.846722	40.218356
3149.405544	645326.016060	40.223373
3152.489562	646411.918515	40.228391
3155.636367	647488.094177	40.233408
3158.479396	648575.865694	40.238426
3161.824074	649663.777369	40.243444
3164.987231	650751.985225	40.248461
3168.088708	651837.490417	40.253479
3171.113194	652933.504024	40.258496
3174.062497	654031.184150	40.263514
3177.154148	655119.276600	40.268532
3180.595780	656233.341288	40.273549
3183.326982	657344.599594	40.278567
3186.448774	658443.252978	40.283584
3189.268236	659566.180888	40.288602
3192.151321	660678.588466	40.293620
3195.334435	661809.858269	40.298637
3198.471264	662940.693203	40.303655
3201.979757	664071.622767	40.308672
3204.583064	665200.912238	40.313690
3208.231802	666337.974536	40.318708
3211.742281	667473.175679	40.323725
3215.120499	668599.724348	40.328743
3218.725146	669720.094981	40.333760
3222.175702	670857.193477	40.338778
3225.373957	671982.835621	40.343796
3228.858067	673101.845911	40.348813
3232.257333	674217.454668	40.353831
3235.451332	675328.492945	40.358848
3238.313284	676409.923799	40.363866
3241.403376	677498.312254	40.368884
3244.696276	678574.697083	40.373901
3247.706996	679661.880253	40.378919
3250.936174	680732.753708	40.383936
3253.566171	681813.730603	40.388954
3256.784641	682921.049732	40.393972
3260.022199	684022.529977	40.398989
3263.185243	685126.894759	40.404007
3266.416367	686232.784693	40.409024
3269.499327	687343.447319	40.414042
3272.592075	688462.515009	40.419060
3276.235755	689576.054869	40.424077
3278.743134	690714.143448	40.429095
3281.998182	691841.577499	40.434112
3285.289111	692990.548440	40.439130
3288.710662	694146.602184	40.444148
3292.301853	695287.445201	40.449165
3295.382724	696449.402240	40.454183
3298.980579	697604.196892	40.459200
3302.068078	698763.598733	40.464218
3305.237253	699943.512478	40.469236
3308.683891	701113.779570	40.474253
3311.890868	702290.627679	40.479271
3315.356878	703470.322808	40.484288
3318.461704	704661.004627	40.489306
3321.789404	705849.351862	40.494324
3325.423348	707041.963268	40.499341
3328.601578	708247.341668	40.504359
3331.890449	709466.723882	40.509376
3335.359332	710687.664589	40.514394
3338.775193	711888.503596	40.519412
3342.185619	713105.576278	40.524429
3345.634448	714321.763246	40.529447
3349.059650	715525.245738	40.534464
3352.504649	716759.829492	40.539482
3355.534207	717976.150421	40.544500
3359.072859	719197.914530	40.549517
3362.597692	720428.303328	40.554535
3365.857698	721649.278242	40.559552
3369.449635	722893.837583	40.564570
3372.624863	724131.317853	40.569588
3376.542318	725354.108282	40.574605
3379.663032	726595.478264	40.579623
3383.538967	727822.355464	40.584640
3387.217444	729044.439555	40.589658
3391.171146	730277.300684	40.594676
3394.197173	731497.759793	40.599693
3397.405716	732728.809577	40.604711
3401.106331	733963.856817	40.609728
3404.249711	735198.294681	40.614746
3407.656469	736430.618448	40.619764
3411.415397	737658.406764	40.624781
3414.476068	738898.334018	40.629799
3417.842805	740132.699173	40.634816
3420.789014	741366.529581	40.639834
3424.162038	742618.206058	40.644852
3427.384105	743860.853659	40.649869
3431.076007	745118.139293	40.654887
3434.627150	746362.565923	40.659904
3437.541045	747625.035542	40.664922
3441.040434	748881.746621	40.669940
3444.662278	750139.445560	40.674957
3447.745442	751402.746942	40.679975
3450.845455	752669.942046	40.684992
3454.505205	753922.850966	40.690010
3457.610382	755194.793610	40.695028
3461.539926	756446.270404	40.700032
3465.025242	757661.506459	40.705037
3468.760589	758822.460156	40.710042
3472.240529	759915.926777	40.715047
3475.392464	760960.363908	40.720052
3478.611483	761940.657560	40.725056
3481.081797	762856.029093	40.730061
3483.218061	763716.894681	40.735066
3485.846417	764526.924479	40.740071
3488.493636	765285.326622	40.745076
3490.648795	765971.391313	40.750080
3492.675834	766601.765949	40.755085
3494.826612	767186.582372	40.760090
3496.920035	767727.106855	40.765095
3498.039001	768215.300773	40.770100
3500.086583	768648.326977	40.775104
3501.392647	769049.019913	40.780109
3502.908039	769400.756652	40.785114
3504.959482	769716.049191	40.790119
3506.279923	769983.183078	40.795124
3507.561032	770199.652764	40.800128
3508.360438	770396.329605	40.805133
3509.794512	770551.610671	40.810138
3510.862661	770692.381077	40.815143
3511.129958	770786.541136	40.820148
3512.191390	770843.748954	40.825152
3513.366077	770908.686391	40.830157
3514.427959	770930.930155	40.835162
3514.858229	770925.517938	40.840167
3515.110268	770894.634495	40.845172
3515.898521	770848.857896	40.850176
3516.410149	770795.229203	40.855181
3516.790798	770715.140060	40.860186
3517.134382	770623.531686	40.865191
3517.364913	770518.552001	40.870196
3517.489024	770389.557595	40.875200
3518.049704	770266.671726	40.880205
3517.998171	770124.507688	40.885210
3518.208563	769978.523429	40.890215
3518.407433	769816.255124	40.895220
3518.620339	769653.882706	40.900224
3518.818768	769478.511306	40.905229
3518.885825	769297.564486	40.910234
3519.143495	769104.222637	40.915239
3518.977028	768914.865739	40.920244
3518.845261	768715.540597	40.925248
3518.674909	768512.978176	40.930253
3519.050012	768313.758401	40.935258
3518.769809	768090.548486	40.940263
3519.001353	767890.897439	40.945268
3518.939744	767668.375578	40.950272
3519.020353	767462.946706	40.955277
3519.042447	767244.323004	40.960282
3519.182204	767011.494394	40.965287
3518.783992	766784.826239	40.970292
3519.163185	766555.575751	40.975296
3518.908721	766328.085090	40.980301
3518.618915	766099.611066	40.985306
3518.410471	765871.852879	40.990311
3518.205060	765640.651550	40.995316
3518.249029	765400.128208	41.000320
3518.280295	765184.137245	41.005325
3517.670538	764945.319896	41.010330
3517.818991	764714.326885	41.015335
3517.398121	764487.538114	41.020340
3517.474050	764258.259176	41.025344
3517.161575	764048.913008	41.030349
3517.586988	763824.228257	41.035354
3517.567699	763591.358904	41.040359
3517.071249	763368.030773	41.045364
3517.215569	763138.311574	41.050368
3516.888625	762909.836726	41.055373
3516.438372	762690.259863	41.060378
3516.541451	762473.977252	41.065383
3516.441292	762257.768817	41.070388
3516.196472	762025.864456	41.075392
3515.780327	761822.850649	41.080397
3515.652642	761607.510234	41.085402
3515.410676	761392.622996	41.090407
3515.416637	761201.899402	41.095412
3515.415493	760979.939788	41.100416
3514.981017	760776.014572	41.105421
3514.684191	760570.343063	41.110426
3514.670676	760374.001476	41.115431
3514.888027	760182.627788	41.120436
3514.434404	759975.047959	41.125440
3514.298110	759776.056697	41.130445
3513.836917	759581.874913	41.135450
3513.987365	759390.588352	41.140455
3513.861301	759199.978369	41.145460
3513.797595	759012.251598	41.150464
3513.909838	758824.836171	41.155469
3513.308259	758634.383454	41.160474
3513.481727	758452.990732	41.165479
3513.150276	758275.504091	41.170484
3513.303421	758086.687122	41.175488
3513.067524	757911.239716	41.180493
3513.088891	757726.413106	41.185498
3512.419335	757546.946674	41.190503
3512.528032	757375.362553	41.195508
3512.530775	757196.322569	41.200512
3512.446790	757030.803604	41.205517
3511.945393	756864.608981	41.210522
3512.337912	756701.317192	41.215527
3511.821030	756526.763797	41.220532
3511.781513	756356.210024	41.225536
3511.474409	756200.829185	41.230541
3511.424698	756042.800210	41.235546
3511.384518	755886.682776	41.240551
3511.130419	755735.411407	41.245556
3511.020737	755562.736338	41.250560
3510.701385	755423.115784	41.255565
3510.957033	755276.620362	41.260570
3510.777216	755127.978347	41.265575
3510.754807	754981.766049	41.270580
3510.596205	754826.528483	41.275584
3510.607558	754678.338674	41.280589
3510.348323	754527.730484	41.285594
3510.442197	754384.043608	41.290599
3510.208452	754254.118945	41.295604
3509.972965	754099.713142	41.300608
3509.600589	753963.021471	41.305613
3509.475950	753829.876883	41.310618
3509.597515	753692.857026	41.315623
3509.386213	753562.621287	41.320628
3509.222980	753428.885336	41.325632
3509.281322	753304.698496	41.330637
3509.012566	753173.137294	41.335642
3509.042960	753046.295620	41.340647
3508.947887	752930.926256	41.345652
3508.562765	752792.640914	41.350656
3508.813357	752685.964705	41.355661
3508.289885	752570.066502	41.360666
3508.529013	752456.603842	41.365671
3508.495774	752342.542790	41.370676
3508.241738	752219.123400	41.375680
3508.012694	752106.023368	41.380685
3507.916794	752000.177785	41.385690
3507.954057	751886.688469	41.390695
3507.986811	751795.324885	41.395700
3507.891893	751672.657919	41.400704
3507.702452	751574.737270	41.405709
3507.735864	751468.076846	41.410714
3507.642755	751359.270971	41.415719
3507.307906	751259.401792	41.420724
3507.417997	751151.446133	41.425728
3506.997130	751052.325139	41.430733
3506.908628	750964.018801	41.435738
3507.404129	750856.047620	41.440743
3506.697207	750763.606255	41.445748
3506.719285	750672.623442	41.450752
3506.444733	750590.242984	41.455757
3506.939956	750499.429907	41.460762
3506.686218	750400.765571	41.465767
3506.489488	750313.058298	41.470772
3506.480863	750224.927096	41.475776
3506.302891	750142.526399	41.480781
3505.838119	750054.316864	41.485786
3506.977529	749973.773962	41.490791
3506.359796	749898.718315	41.495796
3506.243634	749794.072908	41.500800
3506.095940	749711.416610	41.505805
3506.033045	749633.074429	41.510810
3506.167794	749554.454567	41.515815
3505.816277	749470.450152	41.520820
3505.605160	749386.176870	41.525824
3506.023374	749314.789774	41.530829
3505.719374	749241.498157	41.535834
3505.681322	749162.409142	41.540839
3504.910964	749098.977518	41.545844
3505.272770	749025.923946	41.550848
3505.753591	748951.670465	41.555853
3505.451929	748885.064706	41.560858
3505.406776	748819.303670	41.565863
3505.333331	748743.708152	41.570868
3505.265380	748674.604333	41.575872
3505.782762	748600.636674	41.580877
3505.105843	748534.725838	41.585882
3505.211481	748461.017885	41.590887
3504.862183	748406.664314	41.595892
3505.467973	748330.663120	41.600896
3505.310750	748266.193610	41.605901
3504.888900	748195.271114	41.610906
3504.541104	748123.057252	41.615911
3504.493288	748067.866864	41.620916
3504.625811	748007.679009	41.625920
3504.482562	747959.833000	41.630925
3504.340687	747898.752391	41.635930
3504.429839	747840.537815	41.640935
3504.343327	747796.322482	41.645940
3504.449221	747739.580416	41.650944
3504.271249	747678.159193	41.655949
3504.185835	747622.134894	41.660954
3504.793374	747564.476647	41.665959
3504.499712	747522.948800	41.670964
3504.048463	747460.141646	41.675968
3503.863453	747402.310798	41.680973
3504.117060	747355.136753	41.685978
3504.429502	747313.512953	41.690983
3504.089452	747249.407347	41.695988
3503.928129	747200.132277	41.700992
3503.849104	747158.421174	41.705997
3503.664299	747102.802003	41.711002
3503.957271	747050.305918	41.716007
3503.869435	747015.729815	41.721012
3503.827890	746963.728225	41.726016
3503.479749	746919.302404	41.731021
3503.843115	746875.453944	41.736026
3504.084470	746830.935428	41.741031
3504.000279	746777.709052	41.746036
3504.120569	746728.878797	41.751040
3503.964125	746690.818289	41.756045
3503.610034	746646.932985	41.761050
3503.782684	746584.266714	41.766055
3503.775964	746552.628092	41.771060
3503.479510	746500.958263	41.776064
3504.089713	746455.444850	41.781069
3503.724556	746414.463086	41.786074
3503.702512	746361.912841	41.791079
3503.462064	746324.946112	41.796084
3503.528132	746274.448195	41.801088
3503.445221	746237.013515	41.806093
3503.250652	746200.924735	41.811098
3503.139511	746166.643471	41.816103
3502.941328	746126.421318	41.821108
3502.879946	746082.634460	41.826112
3502.793017	746043.624698	41.831117
3502.570946	746017.971806	41.836122
3502.766599	745982.706719	41.841127
3502.568163	745958.723074	41.846132
3502.442326	745925.870072	41.851136
3502.506067	745896.628896	41.856141
3502.922240	745873.877587	41.861146
3502.877527	745835.204581	41.866151
3502.760905	745811.010812	41.871156
3503.014310	745779.967901	41.876160
3503.041879	745747.040896	41.881165
3502.381968	745718.797943	41.886170
3502.634688	745681.258711	41.891175
3502.271751	745661.187575	41.896180
3502.546475	745629.451713	41.901184
3502.907471	745606.068426	41.906189
3502.834850	745580.390621	41.911194
3502.642147	745537.949756	41.916199
3502.423979	745513.229520	41.921204
3502.739006	745488.278206	41.926208
3502.777779	745464.403484	41.931213
3502.422473	745439.556793	41.936218
3502.802572	745405.933349	41.941223
3502.500984	745385.507358	41.946228
3502.611008	745347.594993	41.951232
3502.444175	745310.217860	41.956237
3502.377939	745295.365322	41.961242
3502.516233	745269.948737	41.966247
3502.287315	745244.884760	41.971252
3502.404584	745216.075412	41.976256
3502.521554	745195.731102	41.981261
3502.604667	745181.051846	41.986266
3502.929135	745152.948095	41.991271
3502.612610	745123.074225	41.996276
3502.571457	745089.515169	42.001280
3502.552597	745062.055335	42.006285
3502.340888	745037.529333	42.011290
3502.722840	745009.809778	42.016295
3502.414988	744982.690121	42.021300
3502.316839	744962.624873	42.026304
3502.487648	744928.982724	42.031309
3502.752485	744912.650340	42.036314
3502.378808	744883.473463	42.041319
3501.942128	744865.823322	42.046324
3501.938892	744854.306851	42.051328
3502.395149	744823.917199	42.056333
3502.379356	744802.558960	42.061338
3502.001662	744778.796307	42.066343
3502.236661	744762.714345	42.071348
3502.048942	744733.901545	42.076352
3502.029309	744709.738160	42.081357
3501.726028	744706.684802	42.086362
3501.771098	744678.081485	42.091367
3502.124772	744667.591747	42.096372
3501.876573	744650.502248	42.101376
3501.465576	744619.066049	42.106381
3501.823190	744621.668031	42.111386
3502.233068	744603.638816	42.116391
3501.874941	744587.058549	42.121396
3501.731408	744565.128943	42.126400
3502.073621	744544.353840	42.131405
3502.217005	744552.452767	42.136410
3501.942407	744519.124451	42.141415
3501.840007	744506.687746	42.146420
3501.862729	744476.462857	42.151424
3502.240530	744470.152812	42.156429
3502.281054	744449.769145	42.161434
3501.991464	744425.450133	42.166439
3501.674180	744407.583327	42.171444
3501.609465	744390.562975	42.176448
3501.829557	744371.086218	42.181453
3501.302259	744366.886424	42.186458
3501.426649	744369.278851	42.191463
3501.611953	744338.978754	42.196468
3501.546968	744325.994455	42.201472
3501.834960	744324.522037	42.206477
3501.998676	744312.929389	42.211482
3502.228677	744292.860214	42.216487
3502.127846	744274.663913	42.221492
3501.844605	744269.982912	42.226496
3502.076119	744238.149292	42.231501
3501.599276	744225.672196	42.236506
3502.162558	744207.568800	42.241511
3501.882518	744203.477924	42.246516
3501.958639	744174.818552	42.251520
3502.186073	744150.270128	42.256525
3501.617495	744140.366809	42.261530
3501.920405	744123.042248	42.266535
3501.885357	744116.599545	42.271540
3501.823700	744096.083192	42.276544
3501.810414	744081.072225	42.281549
3501.395919	744064.499575	42.286554
3501.685147	744059.679723	42.291559
3501.710987	744052.932105	42.296564
3502.028877	744035.358877	42.301568
3502.192686	744027.949762	42.306573
3501.640183	744006.869982	42.311578
3502.106443	743983.563479	42.316583
3501.914205	743973.404205	42.321588
3501.924836	743957.749332	42.326592
3501.828006	743933.300092	42.331597
3501.619525	743923.290959	42.336602
3502.164817	743901.842364	42.341607
3501.656112	743880.558473	42.346612
3501.607677	743875.545162	42.351616
3501.369839	743856.089391	42.356621
3500.947867	743843.110811	42.361626
3501.939174	743841.971376	42.366631
3502.141358	743835.589789	42.371636
3501.892151	743817.021739	42.376640
3502.041909	743801.886258	42.381645
3501.768409	743775.101298	42.386650
3501.790932	743767.123301	42.391655
3501.663889	743748.043724	42.396660
3501.514543	743738.615798	42.401664
3501.690280	743737.062362	42.406669
3501.376728	743716.978122	42.411674
3501.695240	743714.762428	42.416679
3501.620107	743708.965565	42.421684
3501.807303	743693.233297	42.426688
3501.746657	743681.182460	42.431693
3502.060928	743656.864930	42.436698
3501.587311	743637.937694	42.441703
3501.243547	743637.203842	42.446708
3501.696887	743610.895369	42.451712
3501.693549	743610.945145	42.456717
3501.320777	743609.674334	42.461722
3501.735277	743597.253722	42.466727
3501.724139	743577.072595	42.471732
3501.415050	743571.656782	42.476736
3501.685935	743537.106478	42.481741
3501.180630	743529.998364	42.486746
3501.293915	743526.633249	42.491751
3501.330946	743537.703552	42.496756
3501.279747	743511.129003	42.501760
3501.543760	743508.675632	42.506765
3500.886005	743507.597033	42.511770
3501.429640	743500.817187	42.516775
3501.554423	743495.431946	42.521780
3501.258424	743482.186891	42.526784
3501.416577	743478.224012	42.531789
3501.355237	743482.417950	42.536794
3501.323463	743458.941493	42.541799
3501.509065	743445.522630	42.546804
3501.516392	743440.844896	42.551808
3501.432286	743444.254773	42.556813
3501.316735	743413.554813	42.561818
3501.639105	743397.505411	42.566823
3501.556458	743407.610063	42.571828
3501.113247	743387.299042	42.576832
3501.342306	743369.984240	42.581837
3501.201578	743371.286197	42.586842
3501.602162	743363.100974	42.591847
3501.467415	743355.934761	42.596852
3501.181535	743346.921497	42.601856
3501.348661	743333.751458	42.606861
3501.270224	743338.932716	42.611866
3501.000531	743330.753781	42.616871
3501.341722	743317.261132	42.621876
3501.275482	743299.795412	42.626880
3501.513940	743292.521568	42.631885
3501.291836	743304.518849	42.636890
3501.308579	743293.242928	42.641895
3501.295897	743271.781254	42.646900
3501.375338	743275.805616	42.651904
3501.471840	743273.673726	42.656909
3501.211988	743267.659243	42.661914
3501.444809	743247.192922	42.666919
3501.190847	743242.506678	42.671924
3501.223113	743247.375322	42.676928
3501.452740	743242.908854	42.681933
3501.382659	743226.132763	42.686938
3501.611061	743212.756011	42.691943
3501.186843	743205.142611	42.696948
3501.332391	743201.919991	42.701952
3501.322510	743189.712717	42.706957
3501.257767	743184.110728	42.711962
3501.430198	743179.554705	42.716967
3501.423807	743189.204674	42.721972
3501.104668	743173.304293	42.726976
3501.431531	743160.502806	42.731981
3501.480747	743157.689061	42.736986
3501.280509	743153.043590	42.741991
3501.253425	743125.430045	42.746996
3501.425561	743128.455405	42.752000
3501.255579	743126.217440	42.757005
3500.918592	743125.039406	42.762010
3500.900969	743137.054226	42.767015
3501.271986	743128.577986	42.772020
3501.322149	743115.130459	42.777024
3501.489287	743100.187725	42.782029
3500.994495	743100.018953	42.787034
3501.212680	743103.578653	42.792039
3501.224630	743097.521540	42.797044
3501.067566	743080.807942	42.802049
3501.424544	743073.318432	42.807053
3501.049590	743086.029187	42.812058
3501.112161	743086.216353	42.817063
3501.620174	743077.275569	42.822068
3501.469609	743054.554829	42.827073
3501.516653	743053.464440	42.832077
3500.956203	743048.284449	42.837082
3501.474266	743042.837396	42.842087
3501.266950	743029.626883	42.847092
3501.371034	743019.321492	42.852097
3501.217159	743011.961009	42.857101
3501.079650	743021.680928	42.862106
3500.947969	742999.646291	42.867111
3500.708403	742991.511495	42.872116
3500.842780	742981.792082	42.877121
3500.945744	742978.969866	42.882125
3500.982817	742987.333311	42.887130
3501.079848	742985.890483	42.892135
3501.188684	742997.541149	42.897140
3501.077547	742995.589328	42.902145
3501.270141	742985.663898	42.907149
3501.285088	742974.486226	42.912154
3501.207967	742964.799854	42.917159
3501.140159	742963.579713	42.922164
3500.878609	742960.962165	42.927169
3501.269911	742950.365623	42.932173
3501.152614	742965.104005	42.937178
3501.300716	742936.674668	42.942183
3501.330772	742938.097696	42.947188
3501.213573	742931.666787	42.952193
3501.086908	742924.941966	42.957197
3500.898192	742935.703856	42.962202
3501.196172	742929.109580	42.967207
3501.031428	742910.279857	42.972212
3501.142842	742903.665492	42.977217
3501.186500	742893.615525	42.982221
3501.392727	742899.244908	42.987226
3501.368985	742893.783980	42.992231
3501.067572	742877.387868	42.997236
3500.837479	742879.146964	43.002241
3500.890245	742868.357068	43.007245
3501.205612	742878.547927	43.012250
3501.281563	742871.200606	43.017255
3501.008160	742873.064936	43.022260
3501.207247	742875.495412	43.027265
3501.423320	742854.439833	43.032269
3501.454460	742846.705640	43.037274
3501.322945	742846.184680	43.042279
3501.126444	742841.932278	43.047284
3501.357473	742834.659141	43.052289
3501.572753	742816.065158	43.057293
3501.059497	742814.373076	43.062298
3501.213871	742823.210690	43.067303
3501.537190	742820.993979	43.072308
3501.175171	742799.093207	43.077313
3501.210693	742786.090450	43.082317
3501.175264	742782.157457	43.087322
3501.176000	742779.301913	43.092327
3501.116808	742785.317500	43.097332
3501.081730	742769.322598	43.102337
3501.102080	742752.580513	43.107341
3500.896957	742759.455881	43.112346
3500.983746	742757.522287	43.117351
3501.527677	742760.637377	43.122356
3501.182178	742758.131343	43.127361
3501.234416	742739.661117	43.132365
3501.196796	742743.605609	43.137370
3501.139635	742743.811502	43.142375
3501.291590	742737.387578	43.147380
3501.094799	742739.830753	43.152385
3501.421355	742725.896212	43.157389
3500.799372	742723.187225	43.162394
3500.875594	742718.793652	43.167399
3500.992449	742718.775413	43.172404
3501.064265	742712.708623	43.177409
3501.507469	742716.282570	43.182413
3500.736575	742720.390936	43.187418
3501.313820	742708.435702	43.192423
3501.185709	742693.242897	43.197428
3500.955093	742682.940121	43.202433
3501.142911	742686.061679	43.207437
3501.085996	742678.784168	43.212442
3500.983974	742682.197201	43.217447
3500.783602	742686.561027	43.222452
3500.978190	742693.620136	43.227457
3501.142952	742667.698010	43.232461
3501.040641	742663.824642	43.237466
3501.483464	742659.422957	43.242471
3501.493401	742656.516695	43.247476
3500.927006	742654.488251	43.252481
3501.181060	742645.734341	43.257485
3501.523255	742631.107914	43.262490
3500.959224	742617.361620	43.267495
3501.170349	742627.175262	43.272500
3500.908572	742625.886921	43.277505
3501.282296	742618.985127	43.282509
3501.182145	742611.665075	43.287514
3501.243154	742599.248799	43.292519
3501.003047	742595.692335	43.297524
3501.141837	742607.732807	43.302529
3501.220939	742601.073987	43.307533
3500.926721	742607.864958	43.312538
3501.067585	742597.405523	43.317543
3501.213607	742585.369801	43.322548
3500.853806	742576.514835	43.327553
3501.577143	742568.622907	43.332557
3501.321877	742570.041377	43.337562
3501.037587	742563.094695	43.342567
3501.232433	742543.420076	43.347572
3501.729669	742541.176095	43.352577
3501.253790	742537.262589	43.357581
3501.402126	742534.580811	43.362586
3501.398782	742507.552022	43.367591
3501.517163	742507.976649	43.372596
3501.142596	742513.795591	43.377601
3501.008682	742502.345064	43.382605
3501.012199	742507.907971	43.387610
3501.286625	742477.635448	43.392615
3501.166601	742475.980281	43.397620
3501.209564	742478.681467	43.402625
3501.183428	742475.386898	43.407629
3501.686093	742481.511839	43.412634
3501.352306	742452.959015	43.417639
3501.547497	742450.072944	43.422644
3501.123687	742443.394130	43.427649
3501.244469	742447.757128	43.432653
3501.048399	742426.912449	43.437658
3501.331090	742419.433887	43.442663
3501.059146	742417.507048	43.447668
3501.027631	742419.727554	43.452673
3501.354217	742422.335189	43.457677
3501.629425	742419.338129	43.462682
3501.377975	742395.646419	43.467687
3501.389457	742390.524251	43.472692
3501.216325	742387.597264	43.477697
3501.685791	742360.494020	43.482701
3501.221065	742355.249330	43.487706
3501.353547	742345.824779	43.492711
3501.650179	742344.547563	43.497716
3501.196297	742333.343729	43.502721
3501.201181	742327.434788	43.507725
3501.375632	742318.840637	43.512730
3501.710330	742313.963299	43.517735
3501.655717	742303.829414	43.522740
3501.284708	742293.794210	43.527745
3501.400338	742284.864568	43.532749
3501.688342	742274.627847	43.537754
3501.322010	742258.732845	43.542759
3501.469669	742259.152911	43.547764
3500.955848	742255.097476	43.552769
3501.451822	742235.276484	43.557773
3501.103233	742244.193426	43.562778
3501.409522	742236.710989	43.567783
3501.055856	742228.691647	43.572788
3501.101902	742231.343207	43.577793
3501.346386	742209.395087	43.582797
3501.716954	742202.690341	43.587802
3501.022679	742199.500095	43.592807
3501.288993	742197.685998	43.597812
3501.029912	742178.770662	43.602817
3501.446165	742165.461103	43.607821
3501.222546	742168.253313	43.612826
3501.255896	742160.468813	43.617831
3501.425071	742159.802325	43.622836
3501.239605	742146.586795	43.627841
3501.427362	742137.596462	43.632845
3501.522134	742136.301529	43.637850
3500.891530	742137.729519	43.642855
3501.427520	742123.514911	43.647860
3500.947686	742105.667861	43.652865
3501.515109	742092.383774	43.657869
3500.978835	742101.773358	43.662874
3501.219588	742110.007494	43.667879
3501.462675	742089.979460	43.672884
3501.083672	742077.581847	43.677889
3501.320641	742061.050498	43.682893
3501.139544	742079.296456	43.687898
3501.160270	742078.406983	43.692903
3501.328031	742061.344850	43.697908
3501.594480	742050.520344	43.702913
3501.089929	742029.673517	43.707917
3501.096000	742041.489486	43.712922
3501.065785	742034.994951	43.717927
3501.476265	742020.996714	43.722932
3501.323775	742016.983134	43.727937
3501.372930	742009.048290	43.732941
3501.374570	742008.752639	43.737946
3501.570076	742002.616687	43.742951
3501.251739	741969.382014	43.747956
3501.021196	741979.905659	43.752961
3501.095640	741976.447431	43.757965
3500.746382	741977.092906	43.762970
3501.126777	741974.325410	43.767975
3501.418676	741969.405298	43.772980
3500.913638	741952.152660	43.777985
3501.098046	741949.858931	43.782989
3501.336012	741950.560324	43.787994
3501.145511	741952.658112	43.792999
3501.079150	741945.922960	43.798004
3501.047501	741936.178876	43.803009
3501.290366	741913.097654	43.808013
3501.151152	741916.615333	43.813018
3500.944102	741914.235074	43.818023
3501.146020	741917.994851	43.823028
3501.174383	741921.929471	43.828033
3501.043054	741908.803524	43.833037
3500.987285	741900.983441	43.838042
3501.055002	741894.374996	43.843047
3500.938585	741894.245509	43.848052
3501.081701	741891.515075	43.853057
3501.088413	741895.059190	43.858061
3500.782736	741895.057765	43.863066
3500.960041	741894.734649	43.868071
3501.021129	741895.266745	43.873076
3500.842563	741881.360325	43.878081
3500.841305	741872.005309	43.883085
3501.013866	741862.820062	43.888090
3501.001960	741869.518344	43.893095
3500.951065	741858.940117	43.898100
3500.707014	741864.148309	43.903105
3500.969314	741863.368760	43.908109
3500.882100	741873.870152	43.913114
3501.101411	741865.563886	43.918119
3501.554554	741878.098041	43.923124
3501.250163	741860.666107	43.928129
3501.208378	741831.868254	43.933133
3501.350645	741839.576469	43.938138
3501.427993	741837.299441	43.943143
3501.439790	741828.927097	43.948148
3500.896563	741819.016636	43.953153
3501.459167	741800.513494	43.958157
3501.258000	741810.835835	43.963162
3501.265592	741806.501683	43.968167
3501.001299	741786.650612	43.973172
3500.788741	741787.422450	43.978177
3501.193859	741783.272334	43.983181
3500.835855	741788.301438	43.988186
3501.041410	741785.659681	43.993191
3501.195494	741787.211262	43.998196
3500.921648	741793.458174	44.003201
3500.911761	741789.126744	44.008205
3500.850267	741797.999346	44.013210
3500.652986	741787.443899	44.018215
3501.145309	741779.291812	44.023220
3501.122140	741775.307121	44.028225
3501.313867	741757.501952	44.033229
3501.187799	741762.691772	44.038234
3500.654845	741759.328392	44.043239
3500.792692	741763.639894	44.048244
3500.906820	741768.201295	44.053249
3501.227848	741763.571925	44.058253
3500.854962	741768.652608	44.063258
3500.901065	741752.839746	44.068263
3500.996625	741735.985097	44.073268
3500.778787	741731.587663	44.078273
3501.231400	741736.440844	44.083277
3501.299658	741735.740855	44.088282
3501.269897	741740.570962	44.093287
3501.145282	741742.855466	44.098292
3500.914685	741729.892432	44.103297
3501.110505	741710.018465	44.108301
3501.250021	741718.859740	44.113306
3501.146603	741710.209836	44.118311
3501.492323	741712.125389	44.123316
3501.289667	741709.695136	44.128321
3501.330699	741679.554277	44.133325
3501.045208	741684.621356	44.138330
3500.851988	741679.924605	44.143335
3501.218277	741673.909399	44.148340
3501.282399	741684.978277	44.153345
3501.317989	741669.216117	44.158349
3501.047504	741660.001396	44.163354
3501.208771	741658.548267	44.168359
3501.172727	741655.845753	44.173364
3500.803147	741646.449547	44.178369
3501.090010	741649.851507	44.183373
3501.200962	741657.269372	44.188378
3500.859017	741632.801500	44.193383
3501.215343	741617.875406	44.198388
3500.948827	741617.326219	44.203393
3501.354031	741621.743730	44.208397
3500.737522	741614.207957	44.213402
3500.983955	741622.441756	44.218407
3501.113728	741625.425127	44.223412
3500.883328	741629.548075	44.228417
3501.076408	741619.522239	44.233421
3500.985872	741605.207613	44.238426
3500.876170	741596.016917	44.243431
3500.933985	741585.618260	44.248436
3500.756962	741600.959607	44.253441
3500.828199	741594.301101	44.258445
3500.934758	741591.280830	44.263450
3501.111632	741593.567490	44.268455
3501.270442	741599.648452	44.273460
3500.861300	741595.970200	44.278465
3500.895597	741588.037223	44.283469
3500.993288	741572.166666	44.288474
3500.924889	741575.624197	44.293479
3500.966713	741570.989113	44.298484
3501.165713	741571.844356	44.303489
3501.246379	741570.797731	44.308493
3501.132830	741573.671439	44.313498
3501.439512	741568.896470	44.318503
3501.496903	741542.740944	44.323508
3501.333366	741542.471095	44.328513
3501.110524	741531.476111	44.333517
3501.309142	741538.338748	44.338522
3501.095601	741516.607875	44.343527
3501.111834	741508.973079	44.348532
3501.240697	741506.786377	44.353537
3501.153255	741511.625652	44.358541
3501.312374	741508.350928	44.363546
3501.224380	741491.573652	44.368551
3501.371443	741480.077599	44.373556
3500.840379	741470.312484	44.378561
3501.095582	741474.113402	44.383565
3500.895340	741473.849289	44.388570
3500.950477	741464.435695	44.393575
3501.004345	741466.298456	44.398580
3501.027691	741486.385083	44.403585
3501.029241	741467.919570	44.408589
3500.868167	741455.733034	44.413594
3500.993768	741454.827091	44.418599
3501.288170	741452.762218	44.423604
3501.261956	741443.509038	44.428609
3501.236688	741451.588540	44.433613
3501.010874	741442.169596	44.438618
3501.256779	741428.737611	44.443623
3501.368957	741417.099189	44.448628
3500.968701	741427.108503	44.453633
3501.278903	741429.275890	44.458637
3500.933166	741426.375498	44.463642
3500.705979	741415.331776	44.468647
3501.009122	741402.777137	44.473652
3500.774968	741402.173633	44.478657
3501.301042	741396.428671	44.483661
3500.849267	741400.241664	44.488666
3500.750877	741401.635830	44.493671
3501.153385	741395.713218	44.498676
3501.032111	741406.171363	44.503681
3501.017048	741409.571393	44.508685
3501.200532	741410.872252	44.513690
3500.798415	741385.280409	44.518695
3500.803459	741380.798678	44.523700
3500.792581	741386.315447	44.528705
3501.042843	741378.151516	44.533709
3501.095001	741381.688776	44.538714
3501.025636	741377.464883	44.543719
3501.041347	741364.758145	44.548724
3501.153942	741373.259356	44.553729
3500.861122	741374.634680	44.558733
3500.857328	741366.855142	44.563738
3500.705597	741365.697093	44.568743
3500.900437	741357.394079	44.573748
3500.661704	741355.461762	44.578753
3500.764828	741347.074590	44.583757
3501.214585	741350.648194	44.588762
3500.625205	741355.270587	44.593767
3501.161735	741353.955702	44.598772
3500.326473	741367.086080	44.603777
3500.777091	741361.943786	44.608781
3500.633736	741357.140548	44.613786
3500.769375	741358.005722	44.618791
3501.181976	741356.365519	44.623796
3500.763325	741365.589927	44.628801
3500.722806	741370.963616	44.633805
3500.756671	741376.128708	44.638810
3501.005555	741370.722506	44.643815
3501.243378	741367.336933	44.648820
3500.998046	741382.098518	44.653825
3501.213911	741366.701457	44.658829
3501.213455	741343.508754	44.663834
3500.888963	741343.559509	44.668839
3501.173642	741336.473469	44.673844
3501.103003	741340.916296	44.678849
3501.070270	741336.834378	44.683853
3501.171713	741346.666890	44.688858
3501.190188	741324.062066	44.693863
3501.125631	741312.845042	44.698868
3500.848099	741311.608166	44.703873
3500.913483	741308.791183	44.708877
3501.001681	741313.652374	44.713882
3501.115311	741313.092978	44.718887
3501.282849	741313.953170	44.723892
3501.161761	741304.813130	44.728897
3501.353224	741283.165977	44.733901
3501.304588	741275.935016	44.738906
3501.244430	741277.766408	44.743911
3501.535172	741271.664201	44.748916
3501.507056	741256.600502	44.753921
3501.165874	741244.589497	44.758925
3501.427473	741243.465299	44.763930
3500.913616	741244.727473	44.768935
3501.156471	741212.928146	44.773940
3500.965115	741212.367177	44.778945
3501.087251	741207.029912	44.783949
3501.562802	741212.323043	44.788954
3501.328628	741214.378624	44.793959
3501.462379	741197.172069	44.798964
3501.081986	741192.799720	44.803969
3500.959181	741182.724184	44.808973
3500.917389	741182.779988	44.813978
3500.852092	741183.528866	44.818983
3500.959450	741180.656030	44.823988
3500.922334	741195.828625	44.828993
3501.031834	741188.671342	44.833997
3501.238811	741184.059439	44.839002
3500.749434	741166.950223	44.844007
3501.176247	741156.985704	44.849012
3501.112648	741164.825299	44.854017
3501.004349	741159.819480	44.859021
3501.135932	741164.427773	44.864026
3500.912099	741163.280962	44.869031
3501.367148	741163.259098	44.874036
3500.877273	741141.028635	44.879041
3501.165330	741140.294231	44.884045
3500.990931	741134.658567	44.889050
3500.801626	741129.123717	44.894055
3500.983940	741134.511988	44.899060
3500.718059	741130.072457	44.904065
3501.020111	741134.555633	44.909069
3501.271462	741133.826966	44.914074
3500.839579	741132.811160	44.919079
3501.041006	741116.578699	44.924084
3501.190443	741112.566664	44.929089
3501.396780	741109.235139	44.934093
3501.284259	741107.430756	44.939098
3501.319467	741108.163930	44.944103
3500.880859	741086.516206	44.949108
3501.075403	741085.796414	44.954113
3501.305546	741080.294443	44.959117
3501.183813	741069.824636	44.964122
3501.160378	741082.976340	44.969127
3501.296486	741065.424403	44.974132
3501.069742	741067.478863	44.979137
3501.056347	741057.927730	44.984141
3501.140018	741043.880235	44.989146
3501.194636	741052.981806	44.994151
3501.010532	741043.161878	44.999156
3501.296797	741052.128751	45.004161
3501.240864	741026.284559	45.009165
3501.290470	741009.583156	45.014170
3501.208357	741019.494046	45.019175
3501.121668	741007.098159	45.024180
3501.102609	741022.859216	45.029185
3500.897014	741003.587769	45.034189
3501.467379	740982.668402	45.039194
3501.098814	740984.351103	45.044199
3500.938381	740974.379650	45.049204
3500.886211	740982.956315	45.054209
3501.090448	740981.200872	45.059213
3501.053561	740984.555267	45.064218
3500.888621	740983.596197	45.069223
3500.635548	740987.624560	45.074228
3500.872583	740982.318414	45.079233
3500.591988	740971.479347	45.084237
3500.995400	740975.109626	45.089242
3501.048236	740961.559235	45.094247
3501.240688	740954.536490	45.099252
3500.824596	740965.632281	45.104257
3500.893106	740967.049682	45.109261
3501.154232	740957.258527	45.114266
3501.214076	740965.522237	45.119271
3501.165206	740960.506991	45.124276
3501.027657	740937.974612	45.129281
3500.808133	740928.209311	45.134285
3500.858044	740926.625713	45.139290
3500.799005	740938.453641	45.144295
3501.152499	740932.686055	45.149300
3500.784900	740938.554391	45.154305
3501.236404	740942.127925	45.159309
3501.111033	740934.563911	45.164314
3501.203138	740946.466687	45.169319
3500.866649	740919.828823	45.174324
3500.892901	740920.120215	45.179329
3500.436413	740917.630887	45.184333
3500.753205	740921.471712	45.189338
3500.821868	740928.699950	45.194343
3501.220254	740918.788797	45.199348
3500.965167	740925.969158	45.204353
3501.141530	740921.411121	45.209357
3500.803640	740924.664864	45.214362
3501.035709	740924.924082	45.219367
3501.119101	740922.793560	45.224372
3501.208488	740920.908323	45.229377
3501.080078	740900.196446	45.234381
3501.063269	740886.115111	45.239386
3501.042013	740893.160461	45.244391
3500.868803	740887.770645	45.249396
3500.996588	740886.864292	45.254401
3501.254727	740890.911281	45.259405
3501.037309	740871.690580	45.264410
3501.074038	740863.263990	45.269415
3501.053954	740852.236287	45.274420
3500.969559	740855.351943	45.279425
3501.003709	740847.713657	45.284429
3501.080010	740856.270388	45.289434
3500.851168	740852.908286	45.294439
3501.199559	740847.732372	45.299444
3501.419252	740836.913388	45.304449
3501.248537	740808.180909	45.309453
3501.666572	740814.025021	45.314458
3501.144800	740818.883403	45.319463
3501.124882	740808.397305	45.324468
3501.304048	740795.614784	45.329473
3500.945085	740788.579590	45.334477
3501.191691	740789.476731	45.339482
3501.167076	740791.007215	45.344487
3500.889366	740791.001411	45.349492
3501.022443	740796.988573	45.354497
3501.021734	740785.662269	45.359501
3501.630049	740757.004790	45.364506
3501.336859	740762.615406	45.369511
3501.196827	740761.652413	45.374516
3501.214635	740761.354184	45.379521
3501.116347	740738.076368	45.384525
3500.857464	740732.749076	45.389530
3500.639454	740735.688687	45.394535
3500.741483	740720.751279	45.399540
3500.964232	740730.910376	45.404545
3500.639625	740726.824499	45.409549
3501.058940	740730.107695	45.414554
3500.447191	740726.165197	45.419559
3500.711102	740730.900815	45.424564
3500.614742	740740.469588	45.429569
3500.820722	740732.607338	45.434573
3501.161228	740733.588299	45.439578
3500.625676	740744.161394	45.444583
3500.850064	740738.807805	45.449588
3501.175622	740728.612307	45.454593
3501.019162	740736.910089	45.459597
3500.940675	740742.191682	45.464602
3500.546725	740732.601124	45.469607
3500.896735	740718.068158	45.474612
3501.059607	740726.513015	45.479617
3500.837461	740723.740757	45.484621
3501.278589	740714.856812	45.489626
3501.049248	740716.862528	45.494631
3501.448499	740721.823225	45.499636
3501.345087	740722.775090	45.504641
3501.664055	740703.913311	45.509645
3501.350976	740689.877915	45.514650
3501.016414	740696.086001	45.519655
3500.916093	740689.108771	45.524660
3500.912681	740685.809844	45.529665
3501.083721	740678.790183	45.534669
3501.486719	740655.286003	45.539674
3501.477840	740659.424108	45.544679
3501.244580	740645.671627	45.549684
3500.899366	740647.843215	45.554689
3501.034002	740639.351816	45.559693
3501.358627	740613.545172	45.564698
3501.222773	740622.578559	45.569703
3500.961182	740615.675716	45.574708
3500.827138	740622.837450	45.579713
3501.145641	740625.003782	45.584717
3501.183588	740619.383773	45.589722
3500.989435	740602.571810	45.594727
3501.117727	740588.417974	45.599732
3500.822003	740581.618927	45.604737
3500.882753	740578.457662	45.609741
3501.611645	740581.298557	45.614746
3500.900743	740585.152474	45.619751
3501.163203	740578.807881	45.624756
3501.147279	740573.442492	45.629761
3500.980169	740560.221225	45.634765
3501.244014	740557.225189	45.639770
3501.028459	740559.622769	45.644775
3501.197382	740549.845486	45.649780
3501.108477	740545.377931	45.654785
3501.103550	740550.352681	45.659789
3501.249001	740536.836275	45.664794
3501.383902	740525.192887	45.669799
3501.142278	740516.809413	45.674804
3501.277460	740520.334110	45.679809
3501.119868	740527.401124	45.684813
3501.322436	740497.525636	45.689818
3501.070580	740500.864609	45.694823
3501.341048	740495.109661	45.699828
3501.381100	740490.523419	45.704833
3500.849474	740464.406878	45.709837
3500.788277	740417.631103	45.714842
3500.960295	740300.294772	45.719847
3501.111245	740155.183097	45.724852
3500.521540	739960.342515	45.729857
3500.286051	739708.111504	45.734861
3500.280364	739408.748594	45.739866
3499.796617	739057.925569	45.744871
3499.122394	738655.491596	45.749876
3499.050956	738216.733450	45.754881
3498.772451	737721.966406	45.759885
3498.084084	737191.411451	45.764890
3497.488823	736610.101744	45.769895
3496.778705	735971.011204	45.774900
3496.507421	735296.658913	45.779905
3495.084474	734575.849465	45.784909
3494.931640	733809.669581	45.789914
3493.742121	733008.276227	45.794919
3493.033980	732150.319239	45.799924
3491.911087	731244.548504	45.804929
3491.042364	730311.061490	45.809933
3490.580740	729322.746774	45.814938
3489.025072	728292.544431	45.819943
3488.396699	727201.719512	45.824948
3487.390570	726079.118386	45.829953
3485.885346	724914.037328	45.834957
3484.921572	723688.426947	45.839962
3483.152722	722448.626670	45.844967
3481.957038	721148.644585	45.849972
3480.620812	719820.463916	45.854977
3479.337821	718453.124882	45.859981
3478.031226	717027.303708	45.864986
3476.348281	715563.479989	45.869991
3474.500636	714070.001452	45.874996
3473.220443	712541.695807	45.880001
3471.568327	710976.169240	45.885005
3470.343387	709359.281514	45.890010
3468.485207	707717.579671	45.895015
3466.924841	706023.744858	45.900020
3464.927090	704300.473023	45.905025
3462.963186	702527.925663	45.910029
3461.164430	700727.436591	45.915034
3458.796375	698903.658984	45.920039
3457.136474	697039.639509	45.925044
3455.141231	695143.094805	45.930049
3452.802588	693225.798106	45.935053
3451.065131	691261.123925	45.940058
3448.744123	689281.646417	45.945063
3446.437728	687257.314658	45.950068
3444.308772	685208.407647	45.955073
3441.928021	683139.044977	45.960077
3440.033460	681025.975191	45.965082
3437.793774	678883.444030	45.970087
3435.534339	676699.267392	45.975092
3432.728066	674509.998654	45.980097
3430.438292	672281.892306	45.985101
3427.984596	670016.617902	45.990106
3425.462764	667743.605990	45.995111
3423.501860	665433.674512	46.000116
3420.973209	663101.146026	46.005121
3418.358322	660736.829004	46.010125
3415.936255	658335.484181	46.015130
3413.015587	655927.052789	46.020135
3410.692726	653477.761571	46.025140
3407.613469	651014.730806	46.030145
3404.997289	648528.748268	46.035149
3402.413982	646020.813668	46.040154
3399.515987	643493.509528	46.045159
3397.087208	640937.032026	46.050164
3394.241399	638354.542157	46.055169
3391.257580	635760.044203	46.060173
3388.382558	633134.986631	46.065178
3385.605234	630496.317578	46.070183
3382.699913	627833.484544	46.075188
3380.179084	625152.783766	46.080193
3376.920922	622436.252431	46.085197
3374.251371	619717.979113	46.090202
3371.253648	616975.125455	46.095207
3368.111123	614214.696082	46.100212
3365.050989	611424.997587	46.105217
3361.867603	608627.899072	46.110221
3358.810384	605815.257673	46.115226
3355.579328	602979.407951	46.120231
3352.824684	600132.948959	46.125236
3350.044759	597264.742307	46.130241
3346.729491	594372.603071	46.135245
3343.268408	591470.233220	46.140250
3340.053575	588549.603057	46.145255
3336.773168	585611.906342	46.150260
3333.849720	582678.928660	46.155265
3330.428472	579722.130463	46.160269
3327.522235	576750.721525	46.165274
3324.158685	573767.960391	46.170279
3320.761110	570752.198834	46.175284
3317.696323	567740.559305	46.180289
3314.110841	564716.967250	46.185293
3310.819802	561672.051846	46.190298
3306.928436	558619.157145	46.195303
3304.037734	555561.250590	46.200308
3300.426046	552480.107993	46.205313
3296.799511	549402.708820	46.210317
3293.436157	546308.854020	46.215322
3289.821060	543209.032535	46.220327
3286.742644	540092.910721	46.225332
3283.049299	536976.367082	46.230337
3279.370318	533859.260751	46.235341
3276.167133	530700.087545	46.240346
3272.575545	527558.743034	46.245351
3269.105123	524407.411388	46.250356
3265.836562	521241.747936	46.255361
3262.191919	518067.587053	46.260365
3258.484059	514889.217815	46.265370
3254.846599	511707.280513	46.270375
3251.545244	508512.106739	46.275380
3247.596851	505316.461455	46.280385
3244.042047	502107.777756	46.285389
3240.864155	498889.692080	46.290394
3236.792532	495669.069059	46.295399
3233.027368	492446.485501	46.300404
3229.767943	489222.018866	46.305409
3226.131706	485992.430537	46.310413
3222.401711	482749.093011	46.315418
3218.636127	479504.782393	46.320423
3215.060329	476249.262039	46.325428
3211.745554	472996.172474	46.330433
3207.379304	469744.111386	46.335437
3204.408016	466474.398097	46.340442
3200.351905	463216.656418	46.345447
3196.858719	459938.416718	46.350452
3192.798728	456656.703767	46.355457
3189.009530	453393.612555	46.360461
3185.528681	450100.154935	46.365466
3181.741007	446824.923909	46.370471
3178.208350	443552.709277	46.375476
3174.324651	440263.356951	46.380481
3170.083788	436978.752045	46.385485
3167.077891	433668.814709	46.390490
3163.135816	430384.505004	46.395495
3159.525492	427083.984982	46.400500
3155.800337	423789.275076	46.405505
3151.868239	420489.298428	46.410509
3148.227277	417180.180689	46.415514
3144.059771	413884.217359	46.420519
3140.238105	410590.888939	46.425524
3136.633651	407283.636834	46.430529
3132.997781	403988.024269	46.435533
3129.173129	400683.132075	46.440538
3125.207952	397380.580223	46.445543
3121.432666	394071.647185	46.450548
3117.815155	390777.818869	46.455553
3113.924817	387480.696188	46.460557
3110.024375	384178.773127	46.465562
3106.197062	380884.283452	46.470567
3102.511944	377576.758580	46.475572
3098.699647	374278.037738	46.480577
3094.411399	370984.021644	46.485581
3090.692784	367695.472018	46.490586
3086.980720	364404.534869	46.495591
3082.981132	361124.122433	46.500596
3079.519575	357837.319181	46.505601
3075.384928	354547.803400	46.510605
3071.813691	351252.517316	46.515610
3067.935665	347979.314140	46.520615
3063.563260	344694.703660	46.525620
3059.762316	341416.043786	46.530625
3056.016083	338145.866999	46.535629
3052.207275	334880.845699	46.540634
3048.281784	331617.666536	46.545639
3044.250842	328366.994449	46.550644
3040.455337	325108.412011	46.555649
3036.615518	321851.585889	46.560653
3032.657403	318598.113995	46.565658
3028.554773	315364.726191	46.570663
3024.428099	312120.474679	46.575668
3020.622775	308882.004934	46.580673
3016.273093	305653.966335	46.585677
3012.812622	302424.157852	46.590682
3008.746229	299208.576041	46.595687
3004.860742	296006.930392	46.600692
3000.958801	292798.389298	46.605697
2996.890563	289594.311151	46.610701
2992.969116	286397.456072	46.615706
2989.129899	283221.947280	46.620711
2984.900614	280044.650261	46.625716
2981.089304	276866.133718	46.630721
2976.725126	273706.621029	46.635725
2972.644656	270537.422234	46.640730
2968.635271	267402.272688	46.645735
2964.688524	264269.277956	46.650740
2960.743297	261137.869637	46.655745
2956.761129	258023.137086	46.660749
2953.193433	254892.243301	46.665754
2948.824932	251793.949959	46.670759
2944.478451	248698.952192	46.675764
2940.673766	245604.807657	46.680769
2936.523414	242526.535812	46.685773
2932.391557	239449.876140	46.690778
2928.604410	236399.820504	46.695783
2924.461493	233342.357894	46.700788
2920.388910	230297.752743	46.705793
2916.331891	227271.929528	46.710797
2912.381622	224240.965468	46.715802
2908.263530	221232.493247	46.720807
2904.139869	218230.219394	46.725812
2899.970347	215245.082849	46.730817
2895.458175	212263.892575	46.735821
2891.467779	209292.810430	46.740826
2887.551747	206347.371536	46.745831
2883.258412	203395.995598	46.750836
2879.559914	200467.798913	46.755841
2875.164444	197542.818866	46.760845
2871.173749	194632.883669	46.765850
2866.978945	191743.237690	46.770855
2862.965592	188857.400260	46.775860
2858.596753	185984.780884	46.780865
2854.160161	183126.994456	46.785869
2850.299847	180289.266436	46.790874
2846.245915	177458.709930	46.795879
2841.881685	174638.963539	46.800884
2837.966791	171841.560918	46.805889
2833.002772	169048.039559	46.810893
2829.418722	166264.783666	46.815898
2825.220804	163502.546599	46.820903
2820.877817	160672.224755	46.825908
2817.164348	157941.447091	46.830913
2812.493241	155227.588606	46.835917
2808.715934	152507.531326	46.840922
2804.562822	149831.084420	46.845927
2800.474336	147150.076607	46.850932
2796.621870	144485.379988	46.855937
2792.497785	141841.287637	46.860941
2788.112024	139183.167163	46.865946
2783.870545	136560.400946	46.870951
2779.775607	133946.704321	46.875956
2775.906921	131344.433731	46.880961
2771.730951	128768.048630	46.885965
2767.666338	126195.389693	46.890970
2763.485565	123636.976060	46.895975
2759.211544	121090.490987	46.900980
2755.150958	118555.799281	46.905985
2750.734990	116047.602305	46.910989
2746.869277	113533.358870	46.915994
2742.803365	111044.888152	46.920999
2738.737735	108591.768613	46.926004
2734.810882	106122.260511	46.931009
2730.697621	103670.107552	46.936013
2726.483248	101232.588936	46.941018
2722.120045	98818.189865	46.946023
2718.228999	96415.475390	46.951028
2714.128397	94021.655568	46.956033
2710.079376	91651.888243	46.961037
2706.356416	89282.419247	46.966042
2701.941911	86922.380549	46.971047
2697.758020	84579.632332	46.976052
2693.788577	82257.783739	46.981057
2689.704988	79960.135849	46.986061
2685.926424	77655.224242	46.991066
2681.718517	75364.122928	46.996071
2677.390210	73103.684853	47.001076
2673.830247	70833.489939	47.006081
2669.199312	68601.544079	47.011085
2665.145945	66362.311216	47.016090
2660.948580	64147.041238	47.021095
2656.928757	61948.140672	47.026100
2652.448152	59764.368727	47.031105
2648.101805	57594.875862	47.036109
2644.533806	55443.170287	47.041114
2640.146272	53314.828815	47.046119
2636.107799	51195.302769	47.051124
2631.866784	49082.141196	47.056129
2627.723358	47002.646725	47.061133
2623.599254	44920.390256	47.066138
2619.100555	42869.667052	47.071143
2614.987909	40831.050354	47.076148
2611.055182	38805.674382	47.081153
2606.625272	36805.010361	47.086157
2602.360473	34810.712571	47.091162
2598.166908	32830.623863	47.096167
2593.657328	30884.938045	47.101172
2589.070385	28940.441019	47.106177
2584.573461	27032.561603	47.111181
2580.951200	25147.394042	47.116186
2576.780291	23270.084265	47.121191
2571.948190	21425.082985	47.126196
2567.762012	19590.116079	47.131201
2562.795510	17787.719024	47.136205
2558.547645	15988.017220	47.141210
2553.823919	14239.322297	47.146215
2548.967912	12506.134297	47.151220
2544.516402	10800.874030	47.156225
2539.362227	9130.324108	47.161229
2534.779858	7475.362283	47.166234
2529.997771	5872.625492	47.171239
2524.094448	4309.688274	47.176244
2516.439618	2834.671407	47.181249
2501.841035	1611.776764	47.186253
2486.528106	496.080542	47.191258
2449.132169	165.627925	47.196263
2409.702587	191.700115	47.201268
2390.126557	191.472215	47.206273
2386.180675	194.984481	47.211277
2391.224538	205.632815	47.216282
2400.033059	210.683807	47.221287
2407.456240	223.649226	47.226292
2412.418077	208.335045	47.231297
2413.984894	206.738989	47.236301
2413.214624	206.546295	47.241306
2410.926410	199.152816	47.246311
2407.278262	198.549767	47.251316
2403.976641	192.615180	47.256321
2400.575075	194.808381	47.261325
2397.408208	186.963889	47.266330
2394.901948	187.998264	47.271335
2391.458935	192.634127	47.276340
2388.849168	184.658192	47.281345
2385.614012	184.386024	47.286349
2382.832634	176.006657	47.291354
2380.059464	176.456346	47.296359
2376.485336	184.238619	47.301364
2373.495657	170.817008	47.306369
2369.769463	180.866249	47.311373
2366.494847	175.019208	47.316378
2364.038304	178.026389	47.321383
2360.441086	183.040735	47.326388
2357.135663	188.746613	47.331393
2353.621278	176.748571	47.336397
2350.686343	184.668142	47.341402
2347.386482	183.887235	47.346407
2343.934820	190.840410	47.351412
2341.089935	176.886773	47.356417
2337.410521	173.906253	47.361421
2334.041503	174.714936	47.366426
2330.820888	177.813185	47.371431
2327.250908	184.566567	47.376436
2324.073679	175.730275	47.381441
2320.391735	180.125114	47.386445
2317.165543	176.557986	47.391450
2313.746928	176.093071	47.396455
2310.389717	179.193712	47.401460
2307.207973	179.884517	47.406465
2303.685151	183.352767	47.411469
2300.269749	177.322124	47.416474
2296.790443	175.117095	47.421479
2293.458467	179.473009	47.426484
2290.505856	171.446340	47.431489
2286.944976	175.217951	47.436493
2283.390231	179.415725	47.441498
2279.512607	169.616482	47.446503
2276.000749	176.787902	47.451508
2273.610740	167.657622	47.456513
2269.155513	176.802181	47.461517
2265.510729	179.030308	47.466522
2261.938654	171.312544	47.471527
2258.864705	176.912624	47.476532
2255.895741	162.633583	47.481537
2252.300162	176.215425	47.486541
2249.069810	165.223398	47.491546
2245.855386	171.924332	47.496551
2241.733983	166.953328	47.501556
2238.475115	167.766953	47.506561
2235.416912	176.813178	47.511565
2231.428718	174.744739	47.516570
2228.544311	159.101515	47.521575
2224.849995	175.891140	47.526580
2221.483086	164.724330	47.531585
2217.741665	171.007834	47.536589
2213.846904	169.658799	47.541594
2210.949378	169.450921	47.546599
2207.163512	167.841234	47.551604
2204.140492	161.189237	47.556609
2200.255510	174.170942	47.561613
2196.871315	169.293427	47.566618
2193.368798	166.551047	47.571623
2189.808275	170.654834	47.576628
2186.606466	153.896993	47.581633
2182.989641	164.150629	47.586637
2179.709686	165.122599	47.591642
2176.111839	155.431500	47.596647
2172.583000	161.349548	47.601652
2169.828530	157.563128	47.606657
2165.717457	163.904481	47.611661
2162.723258	157.149911	47.616666
2158.985732	155.086576	47.621671
2155.089826	160.764659	47.626676
2151.903863	154.112866	47.631681
2147.993433	156.578750	47.636685
2144.617943	163.690896	47.641690
2141.637445	155.703451	47.646695
2137.697666	168.250801	47.651700
2134.663291	162.856654	47.656705
2131.075701	167.116557	47.661709
2127.501220	163.920373	47.666714
2124.624191	161.902752	47.671719
2120.338071	167.619756	47.676724
2117.123856	163.449689	47.681729
2113.495314	164.802097	47.686733
2110.018939	164.956908	47.691738
2106.599733	154.927830	47.696743
2102.779519	159.379167	47.701748
2099.512527	161.159078	47.706753
2095.872405	153.325481	47.711757
2092.925905	159.759892	47.716762
2089.401585	158.080851	47.721767
2085.730091	155.254215	47.726772
2082.288427	151.474103	47.731777
2078.774000	146.398709	47.736781
2075.274410	155.105883	47.741786
2071.756251	160.326241	47.746791
2067.778267	158.237286	47.751796
2064.677161	150.471229	47.756801
2061.164037	149.869318	47.761805
2057.562140	150.540511	47.766810
2053.927771	153.868091	47.771815
2050.419725	156.900652	47.776820
2047.242008	149.013707	47.781825
2043.977813	153.400207	47.786829
2040.597089	162.563371	47.791834
2037.513815	155.458939	47.796839
2033.261055	163.822057	47.801844
2029.644789	158.639222	47.806849
2026.119949	162.693179	47.811853
2022.952428	153.339782	47.816858
2019.332344	149.211114	47.821863
2015.729987	157.848961	47.826868
2012.530557	150.661472	47.831873
2008.749778	152.404741	47.836877
2005.216025	155.045857	47.841882
2001.884736	151.058671	47.846887
1998.062324	155.424961	47.851892
1994.790498	151.450620	47.856897
1991.764462	152.079183	47.861901
1988.237963	159.404827	47.866906
1984.470169	142.976103	47.871911
1981.029337	156.404056	47.876916
1977.314481	153.059047	47.881921
1973.989297	150.301652	47.886925
1970.607695	150.444842	47.891930
1967.502859	146.909467	47.896935
1963.473101	147.865948	47.901940
1959.954056	151.185002	47.906945
1956.497073	149.191742	47.911949
1952.967337	149.867497	47.916954
1949.754209	148.142973	47.921959
1945.808369	146.972880	47.926964
1942.348462	145.657145	47.931969
1939.146768	148.243155	47.936973
1935.453478	146.116033	47.941978
1932.278528	149.131307	47.946983
1928.196573	154.898685	47.951988
1925.254226	148.139249	47.956993
1921.453234	154.868767	47.961997
1917.714797	157.029397	47.967002
1914.699570	155.128378	47.972007
1910.827110	163.552250	47.977012
1907.668602	153.042684	47.982017
1904.161767	151.117355	47.987021
1900.700974	153.800871	47.992026
1897.005280	143.530406	47.997031
1893.389326	151.461709	48.002036
1889.881740	153.677974	48.007041
1886.480520	141.611827	48.012045
1883.107345	139.387173	48.017050
1880.010323	146.604504	48.022055
1875.937379	150.655686	48.027060
1872.824931	144.767634	48.032065
1869.318322	142.247481	48.037069
1865.552917	149.091670	48.042074
1862.398366	135.487275	48.047079
1858.201642	142.272407	48.052084
1854.929073	142.806707	48.057089
1851.929969	142.057988	48.062093
1847.922957	145.216150	48.067098
1844.682570	144.483044	48.072103
1841.123831	146.280211	48.077108
1837.852323	146.953559	48.082113
1834.307997	146.562258	48.087117
1830.458883	145.003740	48.092122
1826.928155	137.580261	48.097127
1823.273006	140.582124	48.102132
1819.804911	139.739125	48.107137
1816.619542	145.416850	48.112141
1813.027856	136.566532	48.117146
1809.748139	139.810211	48.122151
1806.103751	141.364521	48.127156
1802.688962	142.693071	48.132161
1798.893514	138.411594	48.137165
1795.336611	143.707693	48.142170
1792.194446	130.810094	48.147175
1788.448326	138.625746	48.152180
1785.136757	140.115323	48.157185
1781.788386	138.703092	48.162189
1778.338332	136.901805	48.167194
1774.631098	146.211038	48.172199
1770.903260	140.593341	48.177204
1767.815349	146.730403	48.182209
1764.381485	142.436645	48.187213
1760.581026	142.635961	48.192218
1757.090179	147.380719	48.197223
1753.278066	146.484011	48.202228
1750.280444	140.037016	48.207233
1746.658499	143.770882	48.212237
1743.067097	134.578856	48.217242
1739.551188	142.428101	48.222247
1735.944831	142.185751	48.227252
1732.409424	133.446887	48.232257
1729.069063	143.223912	48.237261
1725.451917	142.416927	48.242266
1722.206450	140.903188	48.247271
1718.408008	145.082312	48.252276
1715.728721	142.483357	48.257281
1711.998485	138.995323	48.262285
1708.232968	148.221946	48.267290
1704.608977	143.651072	48.272295
1701.090833	138.652337	48.277300
1697.511023	139.854883	48.282305
1694.110634	133.214675	48.287309
1690.525244	140.188932	48.292314
1687.403565	131.859913	48.297319
1683.688268	149.684316	48.302324
1680.311485	143.869340	48.307329
1676.426858	136.779728	48.312333
1673.005468	138.650368	48.317338
1669.927362	137.569209	48.322343
1665.899508	137.433981	48.327348
1662.592448	140.258028	48.332353
1658.982865	135.703903	48.337357
1655.196749	135.689036	48.342362
1652.047926	129.496704	48.347367
1648.819907	140.777969	48.352372
1645.613008	130.681064	48.357377
1642.055220	128.662563	48.362381
1637.856731	135.656859	48.367386
1634.735190	130.785909	48.372391
1631.183900	133.442540	48.377396
1627.887465	126.061573	48.382401
1624.098644	121.772806	48.387405
1619.941417	133.462103	48.392410
1616.764745	136.022140	48.397415
1613.491901	132.516344	48.402420
1610.125736	131.951700	48.407425
1606.649245	135.049061	48.412429
1602.678698	134.310088	48.417434
1599.411794	127.149141	48.422439
1595.815110	135.305301	48.427444
1592.597245	133.201976	48.432449
1589.361233	132.031660	48.437453
1585.271703	136.841696	48.442458
1581.936350	129.615536	48.447463
1578.346338	137.137891	48.452468
1575.277479	131.594312	48.457473
1571.534805	132.480697	48.462477
1568.061766	143.797167	48.467482
1564.965214	135.571830	48.472487
1560.813869	137.417548	48.477492
1557.457268	128.935519	48.482497
1554.111485	126.599123	48.487501
1550.419213	133.368680	48.492506
1547.202079	135.526936	48.497511
1543.534258	141.628266	48.502516
1540.004520	140.168573	48.507521
1536.812894	132.704793	48.512525
1533.007996	138.805434	48.517530
1529.999579	133.464386	48.522535
1526.052702	135.426814	48.527540
1522.467639	131.517491	48.532545
1519.035748	130.039328	48.537549
1515.567768	139.469373	48.542554
1512.299765	120.814440	48.547559
1507.975950	125.620042	48.552564
1505.022561	130.252273	48.557569
1502.013969	128.233285	48.562573
1497.587417	132.760738	48.567578
1494.374233	129.951180	48.572583
1490.953673	130.942203	48.577588
1487.387221	133.813231	48.582593
1483.927833	131.867973	48.587597
1480.205796	133.232063	48.592602
1477.154707	126.597381	48.597607
1473.413756	127.135511	48.602612
1470.070689	123.368670	48.607617
1467.102483	119.384964	48.612621
1463.078269	126.285599	48.617626
1459.746988	126.506503	48.622631
1455.926459	126.066818	48.627636
1452.102803	126.836206	48.632641
1449.104809	125.467324	48.637645
1445.288859	131.386219	48.642650
1442.119362	122.333939	48.647655
1438.551021	131.956885	48.652660
1434.955353	128.514340	48.657665
1431.580992	126.353307	48.662669
1427.893433	125.456211	48.667674
1424.689437	122.417445	48.672679
1420.719472	127.895373	48.677684
1417.309645	127.135145	48.682689
1414.178335	122.066483	48.687693
1410.352659	123.665125	48.692698
1406.754218	120.267321	48.697703
1403.539668	122.573915	48.702708
1399.927631	126.733456	48.707713
1396.852313	125.560196	48.712717
1393.057956	119.595565	48.717722
1389.581742	117.732072	48.722727
1385.812456	121.077818	48.727732
1382.269370	115.393406	48.732737
1378.804155	118.245457	48.737741
1375.396000	126.754987	48.742746
1372.253422	115.256052	48.747751
1368.557579	121.377636	48.752756
1364.893308	124.099497	48.757761
1361.598679	116.810107	48.762765
1357.832135	121.740509	48.767770
1354.448142	116.739900	48.772775
1350.663037	124.065061	48.777780
1347.149818	119.461178	48.782785
1344.058352	121.489089	48.787789
1340.436440	110.764410	48.792794
1337.231265	110.636577	48.797799
1333.623824	119.582281	48.802804
1329.775324	124.462246	48.807809
1326.525846	118.690764	48.812813
1323.019861	131.103963	48.817818
1319.806072	107.286783	48.822823
1315.813579	129.890877	48.827828
1311.935423	124.357022	48.832833
1308.568439	111.893477	48.837837
1305.140873	123.971690	48.842842
1302.058770	118.034807	48.847847
1298.535458	112.818744	48.852852
1294.974807	116.764625	48.857857
1291.680213	108.621029	48.862861
1287.670249	118.461843	48.867866
1284.474874	114.194216	48.872871
1280.779611	117.550557	48.877876
1277.478404	117.475743	48.882881
1274.180951	112.588172	48.887885
1270.340346	111.237358	48.892890
1266.974301	115.962721	48.897895
1263.272475	116.668815	48.902900
1259.689946	119.393734	48.907905
1256.306986	112.966120	48.912909
1252.818518	116.910206	48.917914
1249.429246	110.812621	48.922919
1245.605357	113.651261	48.927924
1242.291742	111.028363	48.932929
1238.871048	114.591676	48.937933
1235.106459	114.054734	48.942938
1232.276895	111.077645	48.947943
1228.777685	118.759891	48.952948
1224.746632	109.342699	48.957953
1221.474665	114.315944	48.962957
1217.769200	123.507988	48.967962
1214.220880	109.905426	48.972967
1210.529722	110.170098	48.977972
1207.042171	112.971917	48.982977
1203.866772	119.173430	48.987981
1200.020505	110.629009	48.992986
1197.026871	97.945721	48.997991
1193.083321	111.151955	49.002996
1189.456885	114.801279	49.008001
1186.629005	104.537672	49.013005
1182.885212	116.118077	49.018010
1179.423463	109.256731	49.023015
1175.744990	110.003495	49.028020
1172.152267	108.553802	49.033025
1169.154476	106.726226	49.038029
1165.326920	116.870722	49.043034
1162.040093	114.189874	49.048039
1158.203040	116.410500	49.053044
1154.506968	109.965508	49.058049
1151.470863	100.705807	49.063053
1147.664589	115.121290	49.068058
1144.102710	103.023703	49.073063
1140.230015	119.812959	49.078068
1137.136797	114.311322	49.083073
1134.163327	108.015806	49.088077
1130.312998	110.219537	49.093082
1126.685200	103.716413	49.098087
1123.275460	110.372259	49.103092
1119.756705	108.661064	49.108097
1116.036134	99.970456	49.113101
1112.604186	116.883705	49.118106
1109.316135	99.795058	49.123111
1105.716504	108.027743	49.128116
1102.053126	110.572381	49.133121
1098.621837	98.593581	49.138125
1094.926632	112.849315	49.143130
1092.090368	109.031745	49.148135
1088.415117	119.421346	49.153140
1084.780312	121.952026	49.158145
1081.476960	117.384996	49.163149
1077.598562	113.872965	49.168154
1074.210010	113.005123	49.173159
1070.402171	113.585516	49.178164
1067.653810	109.336568	49.183169
1063.884093	105.086180	49.188173
1060.197212	108.694390	49.193178
1056.325228	106.968921	49.198183
1053.173977	107.940074	49.203188
1049.326769	107.821108	49.208193
1046.141312	109.278519	49.213197
1042.538613	105.603114	49.218202
1039.631956	109.041714	49.223207
1035.933321	112.885897	49.228212
1032.598083	111.142837	49.233217
1028.694690	107.302542	49.238221
1024.717396	114.708518	49.243226
1021.505178	104.046398	49.248231
1018.289970	99.895875	49.253236
1014.977190	111.601833	49.258241
1011.276669	105.885279	49.263245
1007.350404	107.211916	49.268250
1004.160602	101.855171	49.273255
1000.508247	100.237709	49.278260
997.185105	104.788753	49.283265
993.776935	102.288322	49.288269
989.818641	110.140595	49.293274
986.508346	89.777793	49.298279
983.317620	99.860590	49.303284
980.208674	112.477457	49.308289
976.383760	106.318479	49.313293
972.504023	112.513277	49.318298
968.827315	101.677132	49.323303
965.506128	108.527970	49.328308
961.776306	102.860321	49.333313
958.506889	104.264465	49.338317
954.767480	103.802787	49.343322
951.750037	96.378420	49.348327
948.378882	106.729930	49.353332
944.647811	109.797762	49.358337
941.060537	106.034561	49.363341
937.088902	111.588852	49.368346
934.416508	100.832754	49.373351
930.704127	106.261029	49.378356
927.171472	110.996764	49.383361
923.793633	98.032060	49.388365
920.136808	109.114856	49.393370
916.773479	98.830793	49.398375
912.938307	95.327889	49.403380
909.212561	104.997765	49.408385
906.053834	97.905591	49.413389
902.614535	105.132450	49.418394
899.208263	97.708875	49.423399
895.825632	96.558593	49.428404
891.969692	106.941736	49.433409
888.540100	100.404518	49.438413
884.879502	102.635582	49.443418
881.601174	98.488667	49.448423
878.005429	106.148163	49.453428
874.705070	111.812503	49.458433
871.015357	99.086487	49.463437
867.079796	108.928440	49.468442
863.857737	105.718697	49.473447
860.550711	110.960135	49.478452
856.802422	97.841496	49.483457
853.896557	100.280260	49.488461
849.956320	109.369966	49.493466
846.221612	96.628863	49.498471
842.867798	105.541318	49.503476
839.312462	115.194028	49.508481
835.998536	103.586118	49.513485
832.879415	107.035899	49.518490
829.357020	100.272789	49.523495
825.541091	105.549634	49.528500
821.891019	104.093240	49.533505
818.354437	102.824723	49.538509
814.791680	106.641378	49.543514
811.794271	103.829917	49.548519
808.079512	105.594921	49.553524
804.314995	108.364317	49.558529
800.638468	113.201720	49.563533
797.055165	117.385439	49.568538
793.905588	102.831618	49.573543
790.459090	98.556046	49.578548
787.087211	105.826168	49.583553
783.684314	103.312338	49.588557
779.775187	109.780730	49.593562
776.743853	95.319140	49.598567
773.072607	101.370624	49.603572
768.948125	105.673899	49.608577
765.810433	100.967158	49.613581
762.393306	105.669037	49.618586
759.039274	103.596824	49.623591
755.637578	107.381950	49.628596
751.646275	101.859749	49.633601
748.281643	98.090238	49.638605
744.991808	104.180081	49.643610
741.243088	108.725085	49.648615
737.953765	104.548308	49.653620
734.237359	104.152720	49.658625
730.944542	95.566154	49.663629
726.957310	103.986206	49.668634
723.847317	90.407008	49.673639
720.423101	96.505245	49.678644
716.994043	101.209007	49.683649
714.023609	92.578290	49.688653
710.257531	103.285944	49.693658
706.340509	96.970674	49.698663
702.762734	100.780228	49.703668
698.960720	96.810311	49.708673
695.723112	92.631782	49.713677
692.192709	101.100526	49.718682
689.085600	96.613656	49.723687
685.523618	92.701069	49.728692
681.646290	95.361626	49.733697
678.118662	93.610865	49.738701
674.898953	96.067194	49.743706
671.468318	94.288590	49.748711
668.017561	99.726604	49.753716
664.467147	103.993802	49.758721
661.207851	96.094888	49.763725
657.310955	104.396412	49.768730
653.914491	100.309216	49.773735
649.968094	98.563938	49.778740
646.837543	93.201220	49.783745
643.529138	90.691630	49.788749
639.474229	92.889626	49.793754
635.895204	100.730079	49.798759
632.982788	95.545177	49.803764
629.112419	103.541995	49.808769
625.627424	90.255695	49.813773
622.124528	95.676578	49.818778
619.171085	95.481090	49.823783
615.450636	95.962556	49.828788
611.944648	98.887691	49.833793
608.840264	98.333026	49.838797
604.593608	92.094744	49.843802
601.157513	94.616625	49.848807
597.954795	95.263789	49.853812
593.928249	102.832656	49.858817
590.556223	86.023195	49.863821
587.209638	92.890773	49.868826
583.540368	97.201923	49.873831
580.035208	93.998663	49.878836
576.845884	91.771010	49.883841
573.506697	95.489456	49.888845
569.910237	100.118244	49.893850
566.486939	89.859557	49.898855
562.760130	94.701752	49.903860
558.961234	104.459128	49.908865
555.844326	97.044166	49.913869
552.236937	104.376555	49.918874
548.693404	102.871949	49.923879
545.156733	96.373797	49.928884
541.593981	97.852501	49.933889
538.072861	96.641786	49.938893
534.729802	91.767983	49.943898
531.083674	97.328391	49.948903
527.665416	90.371936	49.953908
524.221198	91.145538	49.958913
520.858989	93.633728	49.963917
516.959367	96.952748	49.968922
513.576035	98.703921	49.973927
510.498233	108.917856	49.978932
506.812945	99.488011	49.983937
503.468995	86.695382	49.988941
499.271044	100.884479	49.993946
496.334911	93.153323	49.998951
492.771935	97.046056	50.003956
489.150919	97.363302	50.008961
485.629615	86.768823	50.013965
481.846356	95.720167	50.018970
478.533025	89.408533	50.023975
474.969109	95.604661	50.028980
471.267975	88.224297	50.033985
468.084181	94.987320	50.038989
464.652610	96.186075	50.043994
461.130718	94.089650	50.048999
458.164838	92.586353	50.054004
454.104889	97.793985	50.059009
450.442568	97.636820	50.064013
446.788819	99.389244	50.069018
443.459792	92.963021	50.074023
440.198405	96.061879	50.079028
436.134120	97.565396	50.084033
433.405460	88.681787	50.089037
429.937104	104.240448	50.094042
426.374798	97.354054	50.099047
423.110373	99.782670	50.104052
418.998269	96.373986	50.109057
415.291226	104.623712	50.114061
411.950632	98.316373	50.119066
408.397610	91.782881	50.124071
405.214189	95.521279	50.129076
401.660538	98.441301	50.134081
398.243874	91.044886	50.139085
394.411253	98.023460	50.144090
390.583641	103.514270	50.149095
387.398757	92.481156	50.154100
383.810917	93.492445	50.159105
380.727263	98.158034	50.164109
377.024634	102.025229	50.169114
373.471694	95.080446	50.174119
369.794150	95.042758	50.179124
366.604337	95.400077	50.184129
363.015333	92.618171	50.189133
359.618048	87.344807	50.194138
355.566482	94.446277	50.199143
352.404894	92.540233	50.204148
349.236759	97.810694	50.209153
345.929791	93.105324	50.214157
342.074575	100.887896	50.219162
338.730967	96.425552	50.224167
335.327054	89.776987	50.229172
331.409877	100.274310	50.234177
328.250517	94.470135	50.239181
324.277442	96.073311	50.244186
321.358812	94.423452	50.249191
317.941428	89.102633	50.254196
313.695419	97.693086	50.259201
310.165223	86.220554	50.264205
306.358245	93.460900	50.269210
303.051198	89.065613	50.274215
299.791778	98.023547	50.279220
296.342537	100.449521	50.284225
293.296982	98.468373	50.289229
289.967973	98.692499	50.294234
286.337797	94.471224	50.299239
282.283073	101.664970	50.304244
278.685580	97.666370	50.309249
275.505100	93.909334	50.314253
271.945134	96.950617	50.319258
268.421595	94.715323	50.324263
264.839647	91.498915	50.329268
261.347881	90.843706	50.334273
258.202333	88.451125	50.339277
254.174156	89.892119	50.344282
250.379645	92.406998	50.349287
247.575636	90.739210	50.354292
243.987205	99.315264	50.359297
240.746667	88.360542	50.364301
237.448945	93.085020	50.369306
233.273249	94.245409	50.374311
229.918962	88.000410	50.379316
226.029516	90.397292	50.384321
222.897385	89.581353	50.389325
219.477558	99.662275	50.394330
215.824592	91.015300	50.399335
212.643813	91.396570	50.404340
208.882516	91.580880	50.409345
205.846345	89.867217	50.414349
201.798113	88.473460	50.419354
198.015543	89.531149	50.424359
194.692415	87.884593	50.429364
191.213457	91.381455	50.434369
187.737384	89.233674	50.439373
184.190401	94.829295	50.444378
180.958387	95.003465	50.449383
177.843332	90.676228	50.454388
173.423743	98.218246	50.459393
170.384775	92.461715	50.464397
166.591386	104.565891	50.469402
163.210077	102.909478	50.474407
159.789981	97.791632	50.479412
156.351122	107.777482	50.484417
153.190624	92.501181	50.489421
149.414289	91.128127	50.494426
145.894360	96.814437	50.499431
142.765874	93.204334	50.504436
138.819883	105.895581	50.509441
135.655496	95.318120	50.514445
132.086891	91.308733	50.519450
128.432537	95.146314	50.524455
124.784689	97.056132	50.529460
120.719860	92.931503	50.534465
117.553104	96.480722	50.539469
113.995002	91.017521	50.544474
110.903174	101.398269	50.549479
107.224154	94.188623	50.554484
103.570448	101.310121	50.559489
100.414523	92.123417	50.564493
96.948488	100.389277	50.569498
92.996416	90.605970	50.574503
89.374056	92.227068	50.579508
86.042777	100.705939	50.584513
82.723034	101.248234	50.589517
79.413546	87.618338	50.594522
75.765023	93.141321	50.599527
72.377724	97.601477	50.604532
68.601813	104.302369	50.609537
65.770575	92.568583	50.614541
61.977255	101.727300	50.619546
58.227528	107.535071	50.624551
54.727560	96.330010	50.629556
51.050711	98.921452	50.634561
47.718092	94.868801	50.639565
43.827970	97.076041	50.644570
40.273690	94.386913	50.649575
37.302688	87.945903	50.654580
33.716133	94.908204	50.659585
30.382381	86.850393	50.664589
26.861764	94.349699	50.669594
23.184141	101.902084	50.674599
19.509524	99.719041	50.679604
16.293172	97.625550	50.684609
12.707272	91.394789	50.689613
9.429164	91.832511	50.694618
5.725321	96.279012	50.699623
2.557478	93.728670	50.704628