Thu Aug 25 16:58:54 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
1.115311	105.153435	0.000000
1.331878	111.621134	0.005005
1.702791	107.260278	0.010010
1.236022	108.481896	0.015014
1.125127	100.118396	0.020019
0.892280	102.176571	0.025024
0.697418	85.135284	0.030029
0.962075	79.329410	0.035034
0.813883	77.103197	0.040038
-0.034285	56.351929	0.045043
0.097556	50.721900	0.050048
-0.320177	46.585866	0.055053
-0.713865	32.128959	0.060058
-1.038482	30.392308	0.065062
-1.125974	18.358353	0.070067
-1.132161	17.106490	0.075072
-1.969140	6.825650	0.080077
-2.365505	5.027476	0.085082
-2.238195	11.031392	0.090086
-2.429090	-5.140389	0.095091
-3.127103	-6.002278	0.100096
-3.482185	-12.252026	0.105101
-3.299654	-14.545865	0.110106
-3.692101	-10.441043	0.115110
-4.322978	-6.083725	0.120115
-4.504828	-11.370354	0.125120
-5.183154	-2.880035	0.130125
-5.217871	-13.808586	0.135130
-5.335179	-2.685320	0.140134
-5.016114	-13.675631	0.145139
-5.495885	-10.452475	0.150144
-6.056282	-9.703416	0.155149
-5.888980	-9.011426	0.160154
-6.302600	-8.044917	0.165158
-6.817268	-9.267729	0.170163
-7.589330	-5.559011	0.175168
-7.927027	-1.927840	0.180173
-7.598962	-15.260756	0.185178
-7.586940	6.295372	0.190182
-7.876608	-4.374938	0.195187
-7.803111	-7.271794	0.200192
-7.894118	-1.755699	0.205197
-8.674318	-12.232085	0.210202
-9.375312	-1.938025	0.215206
-9.303786	1.037401	0.220211
-9.245519	-3.160547	0.225216
-9.435400	-4.608255	0.230221
-10.297897	-14.208034	0.235226
-10.859471	-1.635753	0.240230
-10.791802	-4.468421	0.245235
-10.983929	1.370406	0.250240
-11.120920	-2.211649	0.255245
-10.834469	-1.851542	0.260250
-10.885379	-6.358252	0.265254
-11.489917	-9.566489	0.270259
-12.167780	-11.181349	0.275264
-12.380439	2.677708	0.280269
-12.582534	-6.522508	0.285274
-12.618123	-4.545873	0.290278
-12.793607	-2.379638	0.295283
-13.217287	-0.361178	0.300288
-13.571151	1.934248	0.305293
-13.791781	-5.383779	0.310298
-14.069919	3.176718	0.315302
-14.046361	-1.987071	0.320307
-14.022164	-0.491206	0.325312
-15.002631	2.085897	0.330317
-15.016026	-9.855242	0.335322
-15.579124	-9.014009	0.340326
-15.444890	-8.721802	0.345331
-15.617189	-12.061039	0.350336
-15.672960	-3.623972	0.355341
-16.039144	-13.801392	0.360346
-16.943699	-3.383688	0.365350
-17.000327	4.838380	0.370355
-16.927980	-7.138341	0.375360
-17.230493	-10.115488	0.380365
-17.141290	-9.885829	0.385370
-17.702967	-3.935317	0.390374
-18.232604	-7.560254	0.395379
-18.219608	-7.695144	0.400384
-18.772075	-3.207741	0.405389
-18.369864	-13.379004	0.410394
-18.734119	0.060874	0.415398
-19.219807	-6.699926	0.420403
-19.441523	-9.259459	0.425408
-19.808652	-3.155931	0.430413
-19.673526	-10.017165	0.435418
-20.139981	-9.535926	0.440422
-21.128267	-2.632714	0.445427
-21.040798	-13.099515	0.450432
-21.525186	-6.999762	0.455437
-20.766432	-6.302367	0.460442
-21.259474	0.368225	0.465446
-21.551547	2.704589	0.470451
-21.717084	-9.427848	0.475456
-22.542143	-1.098036	0.480461
-22.878251	-2.310860	0.485466
-22.616482	-3.690128	0.490470
-22.891242	-7.867531	0.495475
-22.873083	-4.168731	0.500480
-23.615818	-0.407658	0.505485
-23.728291	-9.663043	0.510490
-24.470916	9.331608	0.515494
-24.542160	-2.132232	0.520499
-24.506272	-0.847008	0.525504
-24.589108	3.579469	0.530509
-24.551044	-5.924133	0.535514
-24.899525	0.878833	0.540518
-25.610061	-8.890290	0.545523
-25.796562	0.313913	0.550528
-25.780069	2.839213	0.555533
-25.884298	-0.586622	0.560538
-26.506363	-1.476227	0.565542
-26.441739	1.557228	0.570547
-26.571477	-1.272984	0.575552
-27.847106	0.625863	0.580557
-28.013779	-5.574312	0.585562
-28.379836	4.423661	0.590566
-28.108532	-10.890380	0.595571
-28.250072	-2.344961	0.600576
-28.481479	-8.674198	0.605581
-28.303413	-3.371108	0.610586
-28.406468	-3.994018	0.615590
-29.059211	-12.816733	0.620595
-29.396597	4.428125	0.625600
-29.496681	1.083898	0.630605
-29.736856	-0.580557	0.635610
-30.656774	3.572114	0.640614
-30.920694	-5.526664	0.645619
-31.152803	-1.219171	0.650624
-31.354771	-6.129321	0.655629
-31.173437	1.644169	0.660634
-31.583703	-8.494707	0.665638
-31.374354	-1.611466	0.670643
-31.546351	-6.599079	0.675648
-32.783460	0.931585	0.680653
-32.696427	-9.101711	0.685658
-33.092436	-9.985606	0.690662
-32.913543	-0.553916	0.695667
-32.716044	0.418082	0.700672
-33.799291	2.337407	0.705677
-34.105284	-2.420403	0.710682
-34.866562	0.748787	0.715686
-34.658229	-3.431544	0.720691
-34.624119	-9.536626	0.725696
-34.848762	-1.699527	0.730701
-34.525939	-2.278435	0.735706
-34.870087	5.979192	0.740710
-35.624205	4.705314	0.745715
-35.560310	-2.824974	0.750720
-36.396021	0.963324	0.755725
-36.099593	-8.837024	0.760730
-36.236846	-5.635897	0.765734
-36.652470	-7.611385	0.770739
-37.150956	-9.067686	0.775744
-37.712389	-2.633154	0.780749
-37.649859	-5.075872	0.785754
-38.055504	4.751133	0.790758
-37.914638	-7.179375	0.795763
-37.681865	-4.675309	0.800768
-38.494073	-5.392750	0.805773
-38.701204	-11.330317	0.810778
-39.166073	-2.987340	0.815782
-39.481768	-8.708579	0.820787
-39.282972	-7.983560	0.825792
-39.409586	2.910209	0.830797
-40.127059	-8.113846	0.835802
-40.668050	4.227422	0.840806
-40.597939	-5.012280	0.845811
-40.565376	-2.230068	0.850816
-41.097533	1.668855	0.855821
-41.270034	-3.581273	0.860826
-41.905493	-1.184776	0.865830
-41.925444	-0.223000	0.870835
-42.331386	-8.451630	0.875840
-42.469874	-4.057565	0.880845
-42.036536	-4.277300	0.885850
-42.141539	-4.849284	0.890854
-43.086890	4.157444	0.895859
-42.852826	-2.371279	0.900864
-43.585201	-0.513258	0.905869
-43.732568	-2.603546	0.910874
-44.302959	5.050446	0.915878
-44.616439	0.923402	0.920883
-44.848865	-6.332662	0.925888
-44.851204	7.680104	0.930893
-45.057116	-1.111386	0.935898
-45.165585	9.111986	0.940902
-45.119091	3.982567	0.945907
-45.755363	2.880052	0.950912
-46.445571	-1.909304	0.955917
-46.302001	-4.456469	0.960922
-46.537536	2.449024	0.965926
-46.626143	3.415230	0.970931
-47.166575	0.728464	0.975936
-47.738976	-7.100758	0.980941
-47.632457	0.089662	0.985946
-48.026533	-0.737587	0.990950
-48.196751	-4.747871	0.995955
-47.984656	-8.112536	1.000960
-48.453139	11.579485	1.005965
-48.625550	-5.851205	1.010970
-49.349933	-1.482397	1.015974
-49.524256	-2.429501	1.020979
-49.332634	0.179090	1.025984
-49.720778	-3.066215	1.030989
-49.638726	-6.584511	1.035994
-50.389355	-3.995962	1.040998
-50.898996	-4.526691	1.046003
-51.026982	1.615298	1.051008
-51.005974	5.620539	1.056013
-50.928765	0.843816	1.061018
-51.521650	8.260888	1.066022
-52.028153	1.889331	1.071027
-52.426260	4.207509	1.076032
-52.868023	3.732583	1.081037
-52.766401	-3.743503	1.086042
-52.948543	4.086938	1.091046
-52.631721	1.506299	1.096051
-52.760604	0.219878	1.101056
-53.470825	7.187095	1.106061
-53.834241	-9.027246	1.111066
-54.051567	4.386447	1.116070
-54.113137	-1.516982	1.121075
-54.907215	-3.815988	1.126080
-55.502762	4.443064	1.131085
-55.623992	-8.284775	1.136090
-55.514791	-1.316241	1.141094
-55.252983	-3.505443	1.146099
-55.422915	-3.355404	1.151104
-55.931978	-1.582993	1.156109
-55.887321	-4.760070	1.161114
-56.531962	1.076892	1.166118
-56.999708	-5.335536	1.171123
-56.722781	-2.370150	1.176128
-57.246073	7.487944	1.181133
-57.473326	0.857496	1.186138
-58.343007	10.345921	1.191142
-58.576976	1.919498	1.196147
-58.424719	4.936057	1.201152
-58.635267	-0.346074	1.206157
-58.604324	-0.768516	1.211162
-58.950316	-3.539531	1.216166
-59.411756	-6.248163	1.221171
-59.645963	-5.401513	1.226176
-60.224562	-2.691221	1.231181
-59.889263	-10.071040	1.236186
-60.137360	-7.399878	1.241190
-60.594130	2.653435	1.246195
-60.363203	-16.090134	1.251200
-60.986325	5.090936	1.256205
-61.613226	-11.433295	1.261210
-61.642889	1.663086	1.266214
-61.687649	-0.525537	1.271219
-61.934481	-9.174567	1.276224
-62.736046	2.919624	1.281229
-62.460105	-7.605182	1.286234
-63.233057	0.684829	1.291238
-63.086458	-4.295755	1.296243
-63.104556	0.044645	1.301248
-63.482029	0.398048	1.306253
-63.862750	-7.768092	1.311258
-64.378410	-3.697746	1.316262
-64.779196	-8.842498	1.321267
-64.462053	-1.593333	1.326272
-64.918132	2.163956	1.331277
-64.732250	-3.942761	1.336282
-65.255962	2.935119	1.341286
-66.085574	1.002352	1.346291
-65.914459	-4.532571	1.351296
-66.619648	-0.024399	1.356301
-66.347253	2.109624	1.361306
-66.394306	1.291276	1.366310
-66.540160	4.145736	1.371315
-66.934034	0.202135	1.376320
-67.810826	8.122439	1.381325
-67.733631	-6.076011	1.386330
-67.706394	-2.305867	1.391334
-67.671912	0.273561	1.396339
-68.458623	-14.504530	1.401344
-68.956704	3.986719	1.406349
-68.986545	-2.725280	1.411354
-69.213778	4.362411	1.416358
-69.452870	1.919498	1.421363
-69.120917	-2.663020	1.426368
-69.428986	-0.798715	1.431373
-69.985877	-0.901257	1.436378
-70.673380	-2.777195	1.441382
-70.411124	-5.902945	1.446387
-70.591567	-3.796045	1.451392
-71.136612	-0.126057	1.456397
-71.801653	-7.232074	1.461402
-71.862990	-0.717712	1.466406
-72.227974	0.434169	1.471411
-72.046008	0.215856	1.476416
-72.167678	3.620188	1.481421
-72.433088	2.978424	1.486426
-73.183078	-2.184379	1.491430
-73.326501	0.109712	1.496435
-73.251956	0.430253	1.501440
-73.586544	0.859195	1.506445
-73.550097	-1.566781	1.511450
-74.048299	-3.829887	1.516454
-74.095352	10.155082	1.521459
-74.476157	-3.161677	1.526464
-74.771459	7.720558	1.531469
-74.508218	-0.818572	1.536474
-75.413609	-1.701744	1.541478
-76.142615	-0.543444	1.546483
-75.922186	-2.403457	1.551488
-76.156295	0.218057	1.556493
-76.119770	-0.002778	1.561498
-76.594595	-3.747030	1.566502
-76.982613	1.018330	1.571507
-77.381648	-0.282707	1.576512
-77.659182	7.464604	1.581517
-77.568513	-15.028210	1.586522
-77.664857	-6.923315	1.591526
-77.964210	-8.521547	1.596531
-78.682552	-14.730187	1.601536
-79.402848	1.850157	1.606541
-78.756362	-2.034994	1.611546
-79.287852	4.173384	1.616550
-79.442419	0.233415	1.621555
-79.434616	-5.611278	1.626560
-79.961462	3.753822	1.631565
-79.689747	-3.299659	1.636570
-80.637814	2.708236	1.641574
-81.027628	2.070147	1.646579
-81.090335	-6.686828	1.651584
-81.143013	4.609808	1.656589
-80.933959	-4.756066	1.661594
-80.965791	8.606415	1.666598
-81.991530	2.442773	1.671603
-81.758390	-1.042250	1.676608
-82.040398	0.008045	1.681613
-82.326698	-0.010345	1.686618
-83.439403	3.033578	1.691622
-83.593793	0.248361	1.696627
-83.664849	-1.891849	1.701632
-84.329891	8.251050	1.706637
-83.792594	-4.016822	1.711642
-84.000749	0.770976	1.716646
-83.926676	2.885453	1.721651
-84.318041	0.858709	1.726656
-84.534250	8.884316	1.731661
-84.722871	-0.295861	1.736666
-85.764450	7.669247	1.741670
-86.422176	5.984798	1.746675
-86.197618	-5.443124	1.751680
-86.606812	-2.904908	1.756685
-86.574177	1.003595	1.761690
-86.231243	7.862740	1.766694
-86.924829	0.466964	1.771699
-87.064513	-11.131673	1.776704
-87.152183	-1.063431	1.781709
-87.369563	-6.989898	1.786714
-87.656203	-3.309780	1.791718
-88.017629	-7.283772	1.796723
-88.375173	-4.006999	1.801728
-89.382786	2.775860	1.806733
-89.425335	-4.465660	1.811738
-89.260970	-3.621351	1.816742
-89.628622	-0.928291	1.821747
-89.817838	-12.126858	1.826752
-89.983103	4.059632	1.831757
-89.297924	-6.712796	1.836762
-89.929213	5.889394	1.841766
-90.625378	4.963947	1.846771
-90.634410	5.762660	1.851776
-91.278940	12.036210	1.856781
-91.537511	7.207696	1.861786
-92.250459	8.758955	1.866790
-92.317081	-3.316210	1.871795
-92.648488	0.253864	1.876800
-92.884658	5.966712	1.881805
-92.255563	7.174803	1.886810
-92.511668	-0.653357	1.891814
-92.743793	9.409052	1.896819
-93.181070	-3.500219	1.901824
-94.193193	-0.516349	1.906829
-94.424341	3.734047	1.911834
-94.363694	0.519663	1.916838
-94.675893	7.291635	1.921843
-94.703246	1.189855	1.926848
-94.746888	4.502866	1.931853
-94.842010	-1.189657	1.936858
-95.284489	7.469357	1.941862
-95.869179	3.698026	1.946867
-95.879641	-5.082953	1.951872
-96.436122	5.299199	1.956877
-96.434988	9.788447	1.961882
-96.244895	5.924187	1.966886
-96.883228	12.067052	1.971891
-97.340569	7.991026	1.976896
-97.815741	11.267251	1.981901
-97.876882	0.675037	1.986906
-97.949183	20.339784	1.991910
-97.946563	16.065132	1.996915
-98.137910	11.289264	2.006912
-98.416899	1.439901	2.016909
-97.972921	3.454814	2.026906
-97.435304	5.898550	2.036902
-96.684335	3.648981	2.046899
-96.389818	-1.871124	2.056896
-95.426942	1.817457	2.066893
-95.221400	4.585661	2.076890
-94.998970	3.217203	2.086886
-94.131365	-0.983018	2.096883
-93.853399	-4.321063	2.106880
-93.066698	-1.118064	2.116877
-92.642752	2.328678	2.126874
-92.489027	3.714325	2.136870
-91.806677	1.934843	2.146867
-91.098373	-1.277396	2.156864
-90.526322	0.416505	2.166861
-89.741071	1.177337	2.176858
-89.674070	-2.244862	2.186854
-89.720343	-4.410690	2.196851
-88.408617	-6.146237	2.206848
-87.993980	-1.240836	2.216845
-87.733765	-2.349117	2.226842
-87.438978	-5.807007	2.236838
-86.651706	-2.835349	2.246835
-86.406963	1.444102	2.256832
-85.504967	3.067297	2.266829
-85.114430	2.489797	2.276826
-84.831798	3.161491	2.286822
-83.925416	3.973035	2.296819
-83.386857	-5.269492	2.306816
-83.476544	-3.516251	2.316813
-82.835190	-5.070728	2.326810
-82.383088	1.387375	2.336806
-81.433912	2.116186	2.346803
-81.012447	-3.598041	2.356800
-80.795881	-0.080790	2.366797
-80.381626	-0.823564	2.376794
-79.923962	2.684420	2.386790
-79.167080	7.000835	2.396787
-78.359548	7.105603	2.406784
-78.312759	-2.275282	2.416781
-77.794932	-3.316222	2.426778
-76.900952	-1.045533	2.436774
-76.344699	4.407889	2.446771
-76.549461	3.046179	2.456768
-75.924892	7.614578	2.466765
-75.434343	8.735204	2.476762
-74.415523	5.347597	2.486758
-74.017024	5.643171	2.496755
-73.803074	10.757421	2.506752
-73.049674	5.333306	2.516749
-72.707785	2.653655	2.526746
-72.469853	5.771582	2.536742
-71.573526	4.899418	2.546739
-71.317906	0.782420	2.556736
-70.144663	1.973472	2.566733
-69.599311	4.564887	2.576730
-69.439068	4.337088	2.586726
-69.344255	5.877686	2.596723
-69.034122	4.216717	2.606720
-68.181590	12.354388	2.616717
-67.737719	1.191149	2.626714
-67.065682	10.114212	2.636710
-66.780004	8.184641	2.646707
-66.519118	0.420646	2.656704
-65.394633	-0.696344	2.666701
-65.417838	2.110871	2.676698
-64.223780	-0.667459	2.686694
-64.053810	-0.364587	2.696691
-63.828056	0.924243	2.706688
-63.049797	0.419041	2.716685
-62.626256	-2.067493	2.726682
-62.448135	3.632082	2.736678
-61.337415	-0.840649	2.746675
-61.222323	0.962869	2.756672
-60.702863	-1.963184	2.766669
-59.835374	2.323229	2.776666
-59.391382	-4.747190	2.786662
-59.306399	-6.090943	2.796659
-58.784481	-8.124053	2.806656
-57.955554	-4.240248	2.816653
-57.818061	-8.785399	2.826650
-56.701241	-3.492671	2.836646
-56.628133	3.449309	2.846643
-56.490592	0.313832	2.856640
-55.602206	7.954872	2.866637
-55.158465	7.204310	2.876634
-54.266231	5.442629	2.886630
-54.014794	6.727435	2.896627
-53.487345	5.048254	2.906624
-53.320297	1.547021	2.916621
-52.694449	1.772128	2.926618
-52.379549	-3.567437	2.936614
-51.698460	-0.826227	2.946611
-50.798825	1.760362	2.956608
-50.692288	0.707840	2.966605
-50.277618	-0.307432	2.976602
-49.525481	2.346618	2.986598
-49.225822	-1.932504	2.996595
-48.169913	0.902033	3.006592
-47.699822	1.404971	3.016589
-47.906186	-5.620566	3.026586
-47.338074	6.141317	3.036582
-46.664350	3.026365	3.046579
-46.162304	3.641506	3.056576
-45.011411	-3.010649	3.066573
-45.003955	-5.032841	3.076570
-44.729515	-3.111738	3.086566
-44.058091	-0.749153	3.096563
-43.292424	-10.930094	3.106560
-43.125355	-4.573048	3.116557
-43.144488	-10.560362	3.126554
-42.196300	-6.612879	3.136550
-41.500357	-7.298419	3.146547
-40.666818	-0.462918	3.156544
-40.522487	-4.695526	3.166541
-40.545706	-4.229335	3.176538
-39.724775	1.838360	3.186534
-39.129086	-1.334056	3.196531
-38.103975	-1.028955	3.206528
-38.248099	-4.516277	3.216525
-37.735673	-3.132980	3.226522
-36.851258	-5.425628	3.236518
-36.150687	2.716847	3.246515
-36.024856	0.257953	3.256512
-35.796008	1.010936	3.266509
-34.889072	-5.058126	3.276506
-34.535713	-4.549569	3.286502
-34.274125	-6.326475	3.296499
-33.222120	-1.536775	3.306496
-32.785935	-5.764428	3.316493
-32.812884	-5.573253	3.326490
-32.061784	0.578245	3.336486
-31.216002	-0.662967	3.346483
-31.081989	-4.440960	3.356480
-30.622581	-7.839111	3.366477
-29.911323	-8.137407	3.376474
-29.414918	-12.694444	3.386470
-29.275470	-9.079577	3.396467
-28.739142	-9.477176	3.406464
-28.263274	-9.263415	3.416461
-27.424911	-9.597464	3.426458
-27.153113	-7.713961	3.436454
-26.454697	-5.719904	3.446451
-25.758389	-2.296825	3.456448
-25.744004	-3.996985	3.466445
-25.158923	-2.840483	3.476442
-24.442503	0.544599	3.486438
-24.314700	-2.405618	3.496435
-23.161426	-0.242074	3.506432
-22.981571	0.987425	3.516429
-22.703836	-1.900753	3.526426
-22.189732	-2.503946	3.536422
-21.359096	-5.377383	3.546419
-21.109164	-1.640441	3.556416
-20.332894	-6.206484	3.566413
-19.731796	-5.898302	3.576410
-19.843895	-8.795089	3.586406
-18.757621	-5.569329	3.596403
-18.279704	-3.173254	3.606400
-17.781387	-8.703115	3.616397
-17.655179	-8.668986	3.626394
-17.432230	-8.535973	3.636390
-16.633248	2.305915	3.646387
-15.801588	0.224274	3.656384
-15.306460	-9.873097	3.666381
-15.350018	-3.112411	3.676378
-14.385048	-2.807388	3.686374
-13.755139	0.290306	3.696371
-13.589589	-6.378520	3.706368
-13.127542	-10.461336	3.716365
-12.569226	-7.048314	3.726362
-12.040796	-0.798569	3.736358
-11.312195	-0.408993	3.746355
-10.837050	-4.249939	3.756352
-10.700198	-1.645200	3.766349
-9.937034	-6.129994	3.776346
-9.085662	-4.606564	3.786342
-9.060852	-0.295817	3.796339
-8.677902	-2.582752	3.806336
-7.931688	-5.595017	3.816333
-7.673064	-9.538254	3.826330
-6.848409	-2.907265	3.836326
-6.219850	-16.183866	3.846323
-6.204081	-6.467389	3.856320
-5.995657	-7.339470	3.866317
-5.220221	-4.530674	3.876314
-4.462621	-0.635686	3.886310
-3.698943	17.535770	3.896307
-3.658219	12.365872	3.906304
-3.329770	19.404071	3.916301
-2.735960	27.303528	3.926298
-2.332439	34.824153	3.936294
-1.942174	48.660360	3.946291
-1.468174	51.237624	3.956288
-1.119252	69.765560	3.966285
-0.524901	85.407168	3.976282
-0.025063	105.717168	3.986278
0.000000	119.670880	3.991283
0.536952	137.522369	3.996288
0.689621	154.187546	4.001293
0.652542	150.770143	4.006298
1.197599	152.630508	4.011302
1.021747	154.651284	4.016307
0.946900	166.897482	4.021312
0.993396	174.872514	4.026317
1.288509	177.686385	4.031322
1.482063	185.758606	4.036326
1.439716	179.573686	4.041331
1.559795	177.295936	4.046336
1.088896	185.921526	4.051341
1.024516	177.019181	4.056346
1.522048	180.152520	4.061350
1.590707	181.571831	4.066355
1.699938	171.807041	4.071360
1.933526	174.279368	4.076365
1.690526	173.466402	4.081370
1.616875	162.932991	4.086374
1.526157	156.489899	4.091379
1.227913	156.293041	4.096384
1.025461	152.069467	4.101389
1.000060	171.432813	4.106394
1.756420	173.231599	4.111398
1.244119	176.890162	4.116403
1.366286	175.801678	4.121408
1.516476	171.244432	4.126413
1.060914	173.445079	4.131418
1.561458	176.135013	4.136422
1.589705	188.849135	4.141427
1.439907	181.251008	4.146432
1.457665	177.603540	4.151437
1.403972	178.228921	4.156442
1.487750	176.665553	4.161446
1.853613	192.060312	4.166451
1.542227	189.818525	4.171456
1.888137	195.332664	4.176461
1.319417	193.371647	4.181466
1.645934	202.906870	4.186470
2.210665	202.764628	4.191475
1.955661	187.760672	4.196480
1.732855	175.744648	4.201485
1.137994	185.291346	4.206490
1.688246	191.358773	4.211494
1.502343	202.749183	4.216499
1.808241	206.311193	4.221504
1.694121	203.323474	4.226509
1.732634	205.807388	4.231514
1.535015	205.436572	4.236518
1.676367	200.529519	4.241523
1.965897	210.861496	4.246528
1.805392	201.714767	4.251533
1.751641	206.747353	4.256538
1.848924	206.286038	4.261542
1.931760	219.912300	4.266547
2.314366	212.338311	4.271552
2.084537	209.431997	4.276557
1.807692	203.989342	4.281562
2.225057	196.856011	4.286566
2.185950	200.927666	4.291571
1.935691	204.545177	4.296576
1.993916	197.863594	4.301581
1.713095	215.609169	4.306586
2.260705	201.210289	4.311590
1.853280	211.641975	4.316595
1.922223	210.776968	4.321600
2.030281	205.074685	4.326605
1.837272	207.930239	4.331610
1.946446	199.997292	4.336614
1.726477	206.985849	4.341619
1.913053	202.834189	4.346624
1.854075	207.377203	4.351629
2.102101	230.544974	4.356634
2.569603	225.931668	4.361638
1.802446	224.476311	4.366643
1.898838	232.880159	4.371648
2.212890	218.204641	4.376653
2.233155	229.929768	4.381658
2.518577	230.024281	4.386662
2.240042	227.530564	4.391667
2.267165	231.335579	4.396672
2.208385	220.673251	4.401677
2.349620	230.164752	4.406682
2.743812	225.816039	4.411686
1.869181	222.994932	4.416691
2.340335	216.656776	4.421696
2.536542	230.154549	4.426701
2.201863	222.136109	4.431706
2.735729	219.777702	4.436710
2.234950	215.407862	4.441715
2.045283	209.217540	4.446720
2.102951	217.168694	4.451725
2.289196	231.278646	4.456730
2.401084	225.427057	4.461734
2.503276	227.809246	4.466739
2.388996	230.506932	4.471744
2.739150	224.102308	4.476749
2.650559	235.293991	4.481754
2.890573	231.997675	4.486758
2.749774	222.493500	4.491763
2.078560	210.057319	4.496768
2.191455	218.072587	4.501773
2.332385	227.959612	4.506778
2.210310	226.074145	4.511782
2.533805	232.215081	4.516787
2.708176	233.804497	4.521792
2.394528	231.794018	4.526797
2.708004	245.311395	4.531802
2.685650	231.969923	4.536806
2.304338	232.235341	4.541811
2.409264	233.870441	4.546816
2.523674	231.346794	4.551821
2.637294	232.116809	4.556826
2.723130	232.017962	4.561830
2.180352	243.404201	4.566835
2.444314	234.915464	4.571840
2.774465	234.825795	4.576845
2.674225	238.198341	4.581850
2.838243	239.036391	4.586854
2.532400	238.366148	4.591859
2.658912	231.594757	4.596864
2.620554	232.451860	4.601869
2.382713	230.761705	4.606874
3.134541	245.067795	4.611878
2.915534	240.473463	4.616883
2.615923	240.858960	4.621888
2.776873	231.737782	4.626893
2.736189	236.815786	4.631898
3.145926	251.596269	4.636902
2.683413	253.741067	4.641907
2.985526	257.151817	4.646912
3.182594	240.175527	4.651917
3.021674	239.795796	4.656922
2.571577	236.424105	4.661926
2.681115	244.072909	4.666931
2.908083	253.348505	4.671936
2.880586	257.162083	4.676941
3.121243	255.583619	4.681946
2.973098	247.681477	4.686950
2.905175	256.591982	4.691955
3.023887	258.769102	4.696960
3.377049	257.511539	4.701965
2.779646	250.242947	4.706970
2.931310	237.589230	4.711974
3.172787	254.329173	4.716979
3.090869	256.252984	4.721984
2.939899	258.076880	4.726989
2.735333	259.580136	4.731994
3.590119	259.825891	4.736998
3.101426	263.683257	4.742003
2.980396	261.854571	4.747008
3.151598	259.483378	4.752013
3.091198	253.133578	4.757018
3.013699	255.230707	4.762022
2.978141	259.070859	4.767027
2.821093	262.107453	4.772032
3.255470	254.860700	4.777037
3.551477	255.893211	4.782042
3.462350	253.993087	4.787046
3.165312	270.260587	4.792051
3.126053	259.614161	4.797056
3.396888	259.271188	4.802061
3.280169	259.764075	4.807066
3.397638	254.768998	4.812070
3.324748	258.592853	4.817075
3.169038	254.447354	4.822080
3.474876	259.850730	4.827085
3.300452	266.737259	4.832090
3.577668	255.563511	4.837094
3.328247	260.291405	4.842099
3.215101	257.714822	4.847104
3.603161	255.546938	4.852109
3.250880	257.835819	4.857114
3.557203	254.114649	4.862118
3.595394	262.821865	4.867123
3.488042	250.588380	4.872128
3.472477	250.495930	4.877133
3.164945	260.712672	4.882138
3.572302	259.010011	4.887142
3.666358	259.852696	4.892147
3.104773	258.203771	4.897152
3.017902	266.598382	4.902157
3.199065	263.403032	4.907162
3.533122	258.294924	4.912166
3.370036	260.743992	4.917171
3.641381	264.317755	4.922176
3.514108	263.385410	4.927181
3.028638	266.163408	4.932186
3.395556	268.295312	4.937190
3.607537	265.914564	4.942195
3.180256	260.900432	4.947200
3.487602	277.452902	4.952205
3.809588	291.551125	4.957210
3.550631	289.168230	4.962214
3.869021	293.076322	4.967219
3.994020	290.620612	4.972224
3.422583	275.194751	4.977229
3.385112	285.435634	4.982234
3.832883	282.306079	4.987238
4.098306	286.137045	4.992243
3.592534	277.797365	4.997248
3.556442	283.349238	5.002253
3.424160	287.713928	5.007258
3.939397	287.209272	5.012262
3.763752	287.309586	5.017267
3.395709	294.938324	5.022272
3.392446	298.567776	5.027277
3.551132	303.203264	5.032282
3.901032	294.308719	5.037286
3.757638	294.498894	5.042291
3.858118	289.576074	5.047296
3.903143	277.964117	5.052301
3.901155	296.855685	5.057306
3.752542	282.806276	5.062310
3.670388	286.916333	5.067315
3.935941	292.417783	5.072320
3.824461	285.006601	5.077325
3.659154	294.043116	5.082330
3.729591	305.858511	5.087334
3.751428	314.226621	5.092339
3.852317	319.000886	5.097344
4.080720	318.756311	5.102349
3.821211	321.555862	5.107354
3.901096	305.891879	5.112358
3.869205	311.838581	5.117363
3.886195	312.089052	5.122368
4.301550	310.486375	5.127373
3.776284	315.811174	5.132378
3.816231	309.205181	5.137382
4.121292	315.092763	5.142387
4.204935	320.451876	5.147392
4.057465	309.480680	5.152397
4.254039	310.661654	5.157402
4.188919	309.890415	5.162406
4.467638	315.671390	5.167411
4.187441	316.066503	5.172416
4.399629	315.419498	5.177421
4.120141	313.539703	5.182426
4.295411	316.982993	5.187430
4.022909	314.864815	5.192435
4.133497	308.826736	5.197440
4.092408	321.798596	5.202445
3.849988	323.038862	5.207450
4.162010	313.501656	5.212454
4.173625	320.852615	5.217459
4.639416	329.328347	5.222464
4.322362	319.959307	5.227469
4.282041	319.804294	5.232474
4.500748	315.777291	5.237478
4.310381	324.074247	5.242483
4.336384	316.597217	5.247488
4.151211	314.506486	5.252493
4.076615	324.101458	5.257498
4.194491	331.815433	5.262502
4.596696	343.638985	5.267507
4.083171	346.509977	5.272512
4.222139	342.726422	5.277517
4.339120	341.499532	5.282522
4.588237	340.603125	5.287526
4.547148	346.706308	5.292531
4.496597	347.698208	5.297536
4.934672	354.093324	5.302541
4.557278	353.595643	5.307546
4.490578	343.750754	5.312550
4.591555	349.423544	5.317555
4.352646	353.298742	5.322560
4.749588	345.817366	5.327565
4.228049	353.128484	5.332570
4.689178	348.180779	5.337574
4.624422	352.259651	5.342579
4.616906	357.528651	5.347584
4.714650	344.987712	5.352589
4.422251	353.908126	5.357594
4.713464	351.011902	5.362598
4.238990	354.322879	5.367603
4.623627	346.988967	5.372608
4.567847	342.774005	5.377613
4.644595	353.769009	5.382618
4.604044	345.062169	5.387622
4.820850	350.416246	5.392627
4.610898	361.614367	5.397632
5.174401	351.069602	5.402637
4.531941	352.356729	5.407642
4.573133	346.693352	5.412646
4.458272	352.267080	5.417651
4.484930	364.298186	5.422656
4.989575	366.313608	5.427661
4.651683	368.574938	5.432666
5.070811	369.945679	5.437670
5.233240	362.162509	5.442675
4.737081	358.196882	5.447680
4.765153	342.075900	5.452685
4.983054	351.893985	5.457690
4.926733	346.828033	5.462694
4.911695	345.251658	5.467699
4.813637	345.330324	5.472704
4.927977	349.814580	5.477709
5.035055	367.537496	5.482714
5.326332	358.291426	5.487718
5.326068	349.913639	5.492723
4.733461	356.647419	5.497728
4.794576	349.123744	5.502733
4.618314	347.664381	5.507738
5.043208	359.392636	5.512742
5.120646	372.013758	5.517747
4.950209	369.632802	5.522752
5.221388	371.612035	5.527757
5.030172	373.878859	5.532762
5.094757	366.497007	5.537766
5.318548	380.629668	5.542771
5.171051	375.505226	5.547776
5.427491	380.138073	5.552781
4.932093	361.558523	5.557786
5.005251	360.205616	5.562790
4.784364	379.324563	5.567795
4.957267	367.974094	5.572800
5.370624	371.446533	5.577805
4.856457	381.607132	5.582810
5.292856	378.694484	5.587814
5.105017	381.289820	5.592819
5.021130	373.842639	5.597824
5.151875	372.129522	5.602829
4.653912	382.072441	5.607834
5.096238	367.949359	5.612838
5.117180	373.815035	5.617843
5.209485	379.451227	5.622848
5.285904	382.736008	5.627853
5.145982	396.153690	5.632858
5.393103	396.674998	5.637862
5.555342	403.220920	5.642867
5.571697	392.723893	5.647872
5.251297	383.175004	5.652877
4.864895	391.034456	5.657882
5.076228	389.308710	5.662886
5.752817	395.096977	5.667891
5.322594	403.681495	5.672896
5.424751	397.983239	5.677901
5.407022	400.071019	5.682906
5.715319	395.201033	5.687910
5.187672	405.493476	5.692915
5.379490	407.390232	5.697920
5.400306	401.704720	5.702925
5.226229	402.741288	5.707930
5.270769	402.186989	5.712934
5.126490	400.282835	5.717939
5.388533	401.004291	5.722944
5.671932	409.233383	5.727949
5.622443	403.163404	5.732954
5.808417	398.078458	5.737958
5.516197	404.705078	5.742963
5.379860	397.218648	5.747968
5.531669	402.734789	5.752973
5.302312	417.976223	5.757978
6.102879	419.809240	5.762982
5.601130	417.147983	5.767987
5.816301	412.684901	5.772992
5.689758	407.712195	5.777997
5.558030	404.312736	5.783002
6.069402	404.469928	5.788006
5.728780	401.027267	5.793011
5.653377	399.789386	5.798016
5.796984	389.519202	5.803021
5.665517	399.974201	5.808026
5.666492	413.154679	5.813030
5.926599	411.313718	5.818035
5.653641	424.053055	5.823040
5.696200	424.024265	5.828045
5.853050	420.532130	5.833050
5.936727	422.822331	5.838054
5.789570	424.098299	5.843059
5.481803	430.271769	5.848064
6.279315	433.067078	5.853069
6.039486	431.266480	5.858074
5.896267	423.594449	5.863078
5.664484	428.664484	5.868083
6.064105	435.359892	5.873088
6.015999	424.594526	5.878093
5.814123	433.801363	5.883098
5.881097	426.362161	5.888102
5.670147	432.473005	5.893107
5.825251	425.390167	5.898112
6.099755	425.872383	5.903117
5.613011	432.902826	5.908122
5.936113	429.324528	5.913126
5.883574	434.505690	5.918131
6.215199	441.350964	5.923136
6.128116	425.918687	5.928141
6.042822	436.091217	5.933146
6.249581	422.701050	5.938150
6.048948	428.348353	5.943155
6.211781	427.484443	5.948160
6.039613	430.925244	5.953165
6.132128	433.565249	5.958170
6.327779	421.360105	5.963174
6.055638	427.527992	5.968179
5.872982	425.335610	5.973184
6.247719	421.926399	5.978189
5.979672	424.198940	5.983194
6.046935	429.057599	5.988198
6.452790	431.227717	5.993203
6.224639	426.242451	5.998208
6.367952	419.781578	6.003213
6.158154	424.231215	6.008218
6.145220	426.814972	6.013222
5.868748	435.207731	6.018227
5.936565	438.958956	6.023232
6.368298	446.671263	6.028237
6.446969	456.397322	6.033242
6.586430	441.331347	6.038246
6.416375	438.830095	6.043251
6.011706	434.074970	6.048256
6.246013	428.251592	6.053261
5.971414	431.180078	6.058266
6.024264	427.739039	6.063270
5.938713	441.217842	6.068275
6.485050	453.423857	6.073280
6.602977	444.084677	6.078285
6.172494	442.671465	6.083290
6.155161	427.658544	6.088294
6.501021	434.147233	6.093299
6.175996	424.833171	6.098304
5.976448	419.511220	6.103309
6.056737	442.313230	6.108314
6.528674	439.363365	6.113318
6.297195	436.742019	6.118323
6.114842	430.939628	6.123328
6.297672	432.356890	6.128333
5.883872	438.569123	6.133338
6.193008	447.686409	6.138342
6.610479	452.806589	6.143347
6.732883	449.965274	6.148352
6.623742	433.365819	6.153357
6.644988	435.833487	6.158362
6.396024	434.059631	6.163366
6.301717	425.563661	6.168371
6.182668	435.861706	6.173376
6.578766	424.068094	6.178381
6.481091	436.900202	6.183386
6.305854	431.242234	6.188390
6.166295	428.910217	6.193395
6.420292	433.280861	6.198400
6.232585	428.526546	6.203405
6.224046	431.549391	6.208410
6.352669	434.724759	6.213414
6.236638	433.838101	6.218419
5.942463	422.696826	6.223424
6.036340	420.467444	6.228429
6.009943	436.673709	6.233434
6.457627	430.510003	6.238438
6.257205	434.448793	6.243443
5.900746	435.425351	6.248448
6.110205	430.583497	6.253453
5.910132	435.540994	6.258458
6.125195	425.069763	6.263462
6.035382	431.405243	6.268467
5.763262	429.163601	6.273472
6.005916	427.031135	6.278477
6.041807	426.177623	6.283482
6.346855	437.462785	6.288486
6.104296	435.542388	6.293491
6.242720	452.377760	6.298496
6.308845	455.006084	6.303501
5.915952	446.873273	6.308506
6.553622	450.456119	6.313510
6.246607	454.908340	6.318515
6.310826	458.989175	6.323520
6.742551	447.835392	6.328525
6.158546	439.716709	6.333530
6.155052	431.361536	6.338534
6.033480	423.100801	6.343539
5.892789	423.461402	6.348544
6.200884	432.300424	6.353549
6.501671	452.109693	6.358554
6.346414	450.485673	6.363558
6.404784	429.136336	6.368563
6.077047	432.114278	6.373568
6.451151	432.761228	6.378573
6.262056	434.217780	6.383578
6.371558	430.353399	6.388582
6.260668	421.116524	6.393587
6.364488	428.829579	6.398592
6.356339	429.571224	6.403597
5.969902	434.921764	6.408602
6.320830	429.342713	6.413606
6.852862	428.743670	6.418611
6.349807	428.904775	6.423616
6.405277	432.455447	6.428621
6.297021	428.894113	6.433626
6.178133	420.629794	6.438630
6.241450	422.651093	6.443635
6.104999	437.280019	6.448640
6.480535	425.407367	6.453645
6.045062	421.311991	6.458650
6.228755	423.365051	6.463654
6.507109	426.877636	6.468659
6.510265	430.332097	6.473664
6.686255	417.747209	6.478669
5.858424	423.438995	6.483674
6.556518	423.990888	6.488678
6.413308	430.464452	6.493683
6.193176	423.389786	6.498688
6.300451	412.821552	6.503693
6.355491	405.643665	6.508698
5.974664	395.480958	6.513702
6.381091	413.460746	6.518707
6.299264	420.778930	6.523712
6.238957	417.890314	6.528717
5.881231	419.898486	6.533722
5.811536	415.828060	6.538726
6.208148	425.108804	6.543731
6.440160	432.460080	6.548736
6.337821	430.799296	6.553741
5.946967	434.467357	6.558746
6.362872	425.764892	6.563750
6.230754	426.364603	6.568755
6.328558	426.795408	6.573760
6.414310	423.219497	6.578765
6.307212	432.579167	6.583770
6.173033	420.988868	6.588774
6.278129	424.648825	6.593779
6.285173	431.699980	6.598784
6.352800	421.024055	6.603789
6.293241	431.660800	6.608794
6.205877	424.729852	6.613798
6.178837	432.134371	6.618803
6.071560	428.117289	6.623808
5.863607	422.439139	6.628813
5.939565	439.309597	6.633818
6.424094	435.424422	6.638822
6.334477	434.286845	6.643827
6.128583	423.201342	6.648832
6.470272	420.436408	6.653837
6.305911	432.943594	6.658842
6.358994	423.241250	6.663846
6.737052	424.352666	6.668851
6.198801	418.292821	6.673856
5.925856	411.691521	6.678861
6.012766	430.047265	6.683866
6.193256	422.840224	6.688870
6.630881	423.062756	6.693875
6.224445	423.771889	6.698880
6.211912	418.901542	6.703885
6.145813	430.817509	6.708890
6.401461	432.742234	6.713894
6.387058	429.251619	6.718899
6.577719	427.456340	6.723904
6.044371	402.792273	6.728909
6.100232	404.919146	6.733914
5.790350	405.448629	6.738918
6.283276	421.469104	6.743923
6.199079	428.803481	6.748928
6.177534	436.808274	6.753933
6.111010	427.896649	6.758938
6.231050	433.215291	6.763942
6.377534	426.636856	6.768947
5.842178	433.459774	6.773952
6.297466	423.890570	6.778957
6.284515	428.011964	6.783962
6.348191	422.876568	6.788966
6.332722	423.021390	6.793971
6.208104	433.513302	6.798976
6.447091	434.209897	6.803981
6.252893	436.429738	6.808986
6.353264	423.787089	6.813990
6.273170	417.123932	6.818995
6.152013	427.346370	6.824000
6.250890	427.134744	6.829005
6.554672	431.510243	6.834010
6.330276	417.513731	6.839014
6.087629	408.686660	6.844019
6.101891	412.031806	6.849024
6.422233	400.455729	6.854029
6.185667	403.716784	6.859034
6.306655	395.766080	6.864038
6.319211	392.866052	6.869043
5.900207	394.678172	6.874048
6.313797	398.546061	6.879053
6.157693	415.354777	6.884058
6.137574	407.201544	6.889062
6.577346	418.579483	6.894067
6.170442	410.569110	6.899072
6.137876	401.557262	6.904077
5.778964	412.376945	6.909082
6.054093	423.195371	6.914086
6.095170	428.921865	6.919091
6.078249	429.395957	6.924096
6.449354	425.095107	6.929101
5.843459	424.921137	6.934106
6.180072	423.507964	6.939110
6.536571	428.033394	6.944115
6.177178	433.161390	6.949120
6.575263	433.488197	6.954125
6.196376	433.395722	6.959130
6.138402	429.060857	6.964134
6.064368	426.800834	6.969139
6.129667	433.656195	6.974144
6.237025	434.509460	6.979149
6.391954	433.143735	6.984154
6.329177	430.258669	6.989158
6.137548	429.700241	6.994163
6.394032	435.105076	6.999168
6.594598	430.881567	7.004173
6.137039	433.405272	7.009178
6.236475	428.640770	7.014182
6.166046	429.901553	7.019187
6.128205	432.941645	7.024192
6.499121	429.665914	7.029197
6.317883	431.931182	7.034202
6.210265	429.670093	7.039206
6.498019	430.906394	7.044211
6.151885	421.532364	7.049216
6.246068	412.469012	7.054221
6.050022	423.104991	7.059226
6.299969	426.777056	7.064230
6.335873	420.959455	7.069235
6.191921	423.766226	7.074240
6.466899	417.291053	7.079245
6.196575	418.965981	7.084250
5.925746	409.849087	7.089254
6.062956	421.388333	7.094259
5.943651	429.408439	7.099264
6.547392	428.959518	7.104269
6.350437	429.395376	7.109274
6.304434	429.231761	7.114278
6.445201	419.063249	7.119283
6.312968	416.027710	7.124288
6.101945	404.256467	7.129293
5.970185	413.366883	7.134298
6.445728	421.875934	7.139302
6.646559	416.908881	7.144307
6.041711	412.492020	7.149312
6.290638	396.314239	7.154317
6.173227	404.625113	7.159322
5.830509	399.793850	7.164326
6.254932	412.468205	7.169331
5.912154	413.338212	7.174336
6.476662	418.818170	7.179341
6.356596	436.086346	7.184346
6.161340	431.409146	7.189350
6.429924	434.932755	7.194355
5.907142	432.917054	7.199360
6.376741	423.484818	7.204365
6.142112	424.802966	7.209370
6.214331	425.114390	7.214374
6.544098	427.309084	7.219379
6.306997	431.209326	7.224384
6.122204	427.925748	7.229389
5.819170	430.855525	7.234394
6.368069	421.629172	7.239398
6.281983	423.300545	7.244403
6.291447	432.164209	7.249408
6.502158	421.383604	7.254413
6.343275	432.162467	7.259418
5.982739	415.969425	7.264422
6.170820	419.546774	7.269427
5.799799	429.476158	7.274432
6.327190	427.210491	7.279437
6.302504	432.697345	7.284442
6.219247	435.149749	7.289446
6.142812	423.528254	7.294451
6.055471	432.859517	7.299456
6.197099	433.416338	7.304461
6.323381	436.981226	7.309466
6.066761	438.717287	7.314470
6.534917	427.235095	7.319475
6.367027	428.773749	7.324480
6.380316	419.900244	7.329485
6.189169	426.106062	7.334490
6.309938	428.893504	7.339494
6.685444	434.678337	7.344499
6.131438	418.281480	7.349504
6.142422	415.520904	7.354509
5.754564	417.062383	7.359514
5.605418	428.754071	7.364518
6.394694	422.055942	7.369523
6.170054	431.294818	7.374528
6.081094	430.774090	7.379533
5.905496	431.633722	7.384538
5.871997	431.569392	7.389542
6.200400	431.125644	7.394547
5.920868	432.760886	7.399552
5.883470	433.842482	7.404557
5.909357	443.981778	7.409562
6.064847	448.146389	7.414566
6.292163	458.880577	7.419571
6.137745	460.084916	7.424576
6.376371	458.070141	7.429581
6.481232	450.827480	7.434586
6.465156	454.974680	7.439590
6.321068	437.665665	7.444595
6.038621	445.344333	7.449600
6.218043	434.695177	7.454605
5.845670	450.117239	7.459610
6.190920	454.176188	7.464614
6.360607	452.909393	7.469619
6.073960	459.547815	7.474624
6.133005	457.880727	7.479629
6.294739	457.497895	7.484634
6.503527	457.645547	7.489638
6.630337	463.374439	7.494643
6.073649	455.561527	7.499648
6.173333	447.297752	7.504653
6.479636	450.492741	7.509658
6.318144	447.604155	7.514662
6.204880	432.384789	7.519667
5.922198	433.239053	7.524672
6.041254	446.318793	7.529677
6.440964	456.272970	7.534682
6.627108	456.642477	7.539686
6.385121	450.143883	7.544691
6.342706	440.228694	7.549696
6.393585	433.861395	7.554701
6.050764	437.177070	7.559706
5.892733	442.817703	7.564710
6.139482	435.502196	7.569715
5.984614	431.169856	7.574720
6.496901	452.461474	7.579725
6.353558	461.130789	7.584730
6.016448	447.442989	7.589734
6.388317	438.826514	7.594739
6.348730	442.354115	7.599744
6.461625	433.635846	7.604749
6.464836	428.180881	7.609754
6.271627	435.719008	7.614758
5.842953	423.178235	7.619763
6.190160	442.853666	7.624768
6.336027	434.073280	7.629773
5.743932	435.915688	7.634778
6.303293	444.819755	7.639782
6.890245	445.116970	7.644787
6.355375	444.526898	7.649792
6.229928	427.490227	7.654797
6.355983	433.655840	7.659802
6.408215	434.454465	7.664806
6.050311	431.023998	7.669811
6.143654	435.872245	7.674816
6.451400	434.036473	7.679821
5.975858	438.189218	7.684826
6.017577	432.974999	7.689830
6.222186	434.828624	7.694835
6.266644	439.586452	7.699840
6.312011	437.377325	7.704845
5.970613	435.915353	7.709850
6.188131	426.329617	7.714854
6.412264	434.201000	7.719859
6.303002	442.523269	7.724864
6.250100	437.700373	7.729869
5.838959	433.658131	7.734874
6.288048	437.131312	7.739878
6.311204	434.922501	7.744883
6.300275	441.008335	7.749888
6.429502	438.039398	7.754893
6.350826	433.903935	7.759898
6.106712	440.886874	7.764902
6.179668	440.369251	7.769907
5.931843	439.538045	7.774912
6.129940	433.169827	7.779917
6.515139	439.956085	7.784922
5.687676	447.919471	7.789926
6.636918	445.768045	7.794931
6.440401	452.411326	7.799936
6.332135	434.704383	7.804941
6.336143	440.746747	7.809946
6.364634	444.820521	7.814950
6.489617	440.681621	7.819955
5.864133	438.052403	7.824960
5.929428	426.032201	7.829965
6.212669	440.585879	7.834970
6.366564	445.364528	7.839974
6.527721	429.611771	7.844979
6.320298	430.596616	7.849984
6.091994	432.356714	7.854989
6.207206	428.016861	7.859994
6.359402	432.545828	7.864998
6.479222	432.726403	7.870003
6.246656	440.004935	7.875008
6.110803	433.695368	7.880013
6.166344	433.240587	7.885018
6.358637	438.481469	7.890022
6.406645	435.496783	7.895027
5.911022	441.183982	7.900032
6.204110	440.549608	7.905037
6.110200	439.627846	7.910042
5.915427	436.345830	7.915046
5.749020	436.849671	7.920051
6.170426	454.915742	7.925056
6.422692	455.021779	7.930061
6.094254	455.323210	7.935066
6.437827	459.948753	7.940070
6.692019	459.852002	7.945075
6.080262	454.230782	7.950080
6.481563	447.482697	7.955085
6.465937	439.999482	7.960090
6.594933	436.850242	7.965094
6.245657	437.838330	7.970099
6.396954	436.653514	7.975104
6.128389	441.463551	7.980109
5.938643	445.081121	7.985114
6.034699	441.927549	7.990118
6.178033	440.241356	7.995136
5.902054	437.049941	8.000154
6.018394	434.589160	8.005171
6.096294	444.577666	8.010189
6.268924	447.693808	8.015206
6.439815	465.632966	8.020224
6.191581	451.047956	8.025242
6.350494	446.494527	8.030259
6.480916	454.612896	8.035277
5.961904	446.874197	8.040294
6.103156	447.246565	8.045312
6.015761	460.962718	8.050330
6.486792	451.434197	8.055347
6.374471	459.347605	8.060365
6.537308	467.066427	8.065382
6.708330	452.636632	8.070400
6.427599	448.890541	8.075418
6.217935	442.144786	8.080435
6.405012	427.712495	8.085453
6.141572	430.909581	8.090470
6.251087	426.471193	8.095488
6.132557	434.174126	8.100506
6.427792	441.884815	8.105523
6.423818	446.944190	8.110541
6.181397	448.989279	8.115558
6.541682	444.328561	8.120576
6.383349	442.589309	8.125594
6.361724	434.147839	8.130611
6.344982	449.332977	8.135629
6.396975	453.127581	8.140646
6.548831	453.697101	8.145664
6.565109	452.716282	8.150682
6.290590	436.544885	8.155699
6.534936	437.077823	8.160717
6.183514	440.929321	8.165734
6.170052	439.707010	8.170752
6.353898	452.285600	8.175770
6.161228	458.217139	8.180787
6.404740	460.631059	8.185805
6.323569	467.252028	8.190822
6.920970	460.780599	8.195840
6.198458	470.888218	8.200858
6.294349	457.309631	8.205875
6.504089	470.329144	8.210893
6.513898	464.306383	8.215910
6.736451	469.683720	8.220928
6.444436	464.528755	8.225946
6.415635	465.088712	8.230963
6.883119	463.510179	8.235981
6.581917	458.107348	8.240998
6.703020	450.186304	8.246016
6.568940	440.399150	8.251034
6.300009	443.234184	8.256051
6.040941	446.676738	8.261069
6.462913	456.494578	8.266086
6.776564	463.760581	8.271104
6.629943	471.348010	8.276122
6.379903	463.586096	8.281139
6.659866	465.236916	8.286157
6.250143	467.743720	8.291174
6.561355	459.982232	8.296192
6.740700	471.075164	8.301210
6.622532	463.283121	8.306227
6.844749	465.264880	8.311245
6.389105	463.502782	8.316262
6.277390	451.367366	8.321280
6.536010	450.967111	8.326298
6.454797	464.947384	8.331315
6.763529	466.211846	8.336333
6.375116	471.265190	8.341350
6.560999	466.928436	8.346368
6.366383	467.116744	8.351386
6.466948	461.742480	8.356403
6.849575	471.692724	8.361421
6.340902	472.173235	8.366438
6.363012	463.380917	8.371456
6.474995	467.279733	8.376474
6.762565	462.491548	8.381491
6.675174	463.571924	8.386509
6.325326	474.334364	8.391526
6.621937	462.595709	8.396544
6.606345	472.911303	8.401562
6.234567	472.736050	8.406579
6.456483	464.186981	8.411597
6.590083	471.515911	8.416614
6.400494	468.929490	8.421632
6.984166	487.561385	8.426650
6.629245	482.353155	8.431667
6.887904	467.534078	8.436685
6.828792	474.129502	8.441702
6.912409	467.760661	8.446720
6.437693	474.175051	8.451738
6.447187	472.636719	8.456755
6.682925	472.404149	8.461773
6.729266	492.212143	8.466790
6.936924	476.861407	8.471808
6.921579	466.348738	8.476826
6.673491	461.101685	8.481843
6.873007	466.529968	8.486861
6.563374	466.000997	8.491878
6.626087	463.125739	8.496896
6.902969	464.729704	8.501914
6.700211	461.296440	8.506931
6.704021	459.137309	8.511949
6.918186	476.151362	8.516966
7.035129	463.923307	8.521984
6.565532	460.314102	8.527002
6.347426	479.655434	8.532019
6.963193	485.684375	8.537037
6.850435	484.196754	8.542054
7.058956	492.593236	8.547072
7.184991	481.660776	8.552090
6.899555	481.756017	8.557107
6.945633	472.120499	8.562125
6.383957	466.654335	8.567143
6.525776	469.317719	8.572160
6.978606	481.851030	8.577178
6.740184	485.741636	8.582195
6.995027	484.120679	8.587213
7.138177	490.971596	8.592231
6.951918	479.583141	8.597248
6.553708	475.331590	8.602266
6.702633	484.333850	8.607283
6.982050	491.999703	8.612301
6.885099	496.357294	8.617319
6.800882	491.302306	8.622336
7.046558	492.601896	8.627354
6.784818	501.387643	8.632371
6.976952	490.757245	8.637389
7.009046	496.675671	8.642407
6.890498	494.567264	8.647424
6.748546	496.883794	8.652442
6.884526	507.585913	8.657459
6.843565	495.433070	8.662477
6.705053	502.429108	8.667495
6.868595	496.751477	8.672512
6.630900	496.406894	8.677530
6.592351	498.909194	8.682547
7.010076	495.602767	8.687565
6.940207	492.675693	8.692583
6.966592	488.177732	8.697600
7.063567	494.691904	8.702618
6.638258	499.687921	8.707635
6.901461	502.322824	8.712653
6.950484	502.637059	8.717671
6.699789	495.755702	8.722688
7.130912	500.115761	8.727706
7.139721	502.086779	8.732723
7.092834	494.722210	8.737741
6.961000	499.063176	8.742759
7.026416	499.772474	8.747776
7.199974	500.606838	8.752794
6.768385	504.246848	8.757811
7.458829	491.499729	8.762829
7.330066	500.400339	8.767847
6.731821	496.363161	8.772864
7.001003	498.170307	8.777882
6.971538	501.554807	8.782899
7.046809	499.892558	8.787917
6.942735	506.081629	8.792935
7.225365	516.312653	8.797952
7.375668	508.216594	8.802970
6.898420	507.919011	8.807987
7.018722	511.876494	8.813005
7.158700	515.654170	8.818023
7.074383	528.565163	8.823040
7.353812	516.302147	8.828058
7.348719	519.319915	8.833075
6.996044	507.692429	8.838093
7.096752	506.313371	8.843111
7.617907	510.204891	8.848128
7.824351	501.566710	8.853146
7.225768	509.332266	8.858163
7.332553	490.876239	8.863181
7.336885	498.376913	8.868199
7.432825	492.406919	8.873216
7.248481	489.601923	8.878234
7.115543	496.581307	8.883251
6.875317	488.025740	8.888269
7.062025	498.521090	8.893287
7.208233	501.183791	8.898304
7.165408	487.620604	8.903322
6.966565	499.687989	8.908339
6.860968	494.153514	8.913357
7.025826	499.331617	8.918375
7.088077	510.436608	8.923392
7.047372	514.681250	8.928410
7.220456	529.306539	8.933427
7.309337	519.474941	8.938445
7.234659	519.316254	8.943463
7.222813	521.284199	8.948480
7.472570	516.561884	8.953498
7.083500	527.422020	8.958515
7.549686	514.100952	8.963533
7.498801	525.435117	8.968551
7.329506	521.646305	8.973568
7.603314	518.270904	8.978586
7.480337	508.964811	8.983603
7.155561	497.834732	8.988621
7.372685	506.150978	8.993639
7.134839	505.250997	8.998656
7.176772	505.831431	9.003674
7.223268	521.902968	9.008691
7.126639	520.267650	9.013709
7.410773	521.498101	9.018727
7.476446	520.834585	9.023744
7.658931	525.864768	9.028762
7.519961	527.139420	9.033779
7.626561	519.327915	9.038797
7.841456	525.681611	9.043815
7.522765	511.798712	9.048832
7.688381	493.841548	9.053850
7.610303	499.625758	9.058867
7.294653	496.573092	9.063885
7.285479	493.838479	9.068903
7.449053	492.594739	9.073920
7.435610	495.402373	9.078938
7.239859	496.360873	9.083955
7.571548	496.024907	9.088973
7.228591	499.209217	9.093991
7.118468	500.372051	9.099008
7.897044	499.517943	9.104026
7.064107	503.997163	9.109043
7.363056	504.281707	9.114061
7.673251	519.106411	9.119079
7.390260	513.239963	9.124096
7.445805	515.708588	9.129114
7.549002	524.550776	9.134131
7.645884	521.193629	9.139149
7.728105	519.757506	9.144167
7.313708	516.196445	9.149184
7.774910	509.206697	9.154202
7.457771	513.412599	9.159219
7.392476	506.902975	9.164237
7.498671	503.541216	9.169255
7.510107	509.033694	9.174272
7.393275	520.188841	9.179290
7.808686	515.734061	9.184307
7.536279	521.450896	9.189325
7.640646	515.750973	9.194343
7.445413	519.527522	9.199360
7.529876	521.956904	9.204378
7.572733	516.194034	9.209395
7.491110	511.302737	9.214413
7.464494	520.121081	9.219431
7.104924	526.564785	9.224448
7.078608	533.069886	9.229466
7.284399	527.874775	9.234483
7.393431	523.120860	9.239501
7.464142	527.152387	9.244519
7.241209	540.735204	9.249536
7.641777	542.846816	9.254554
7.451175	551.918088	9.259571
7.849768	554.127841	9.264589
7.835545	547.578642	9.269607
7.322312	554.175821	9.274624
7.715887	549.509859	9.279642
7.965847	553.589047	9.284659
7.890602	550.924739	9.289677
7.762284	552.087271	9.294695
7.849090	554.752975	9.299712
8.120117	555.657277	9.304730
8.008832	542.660197	9.309747
7.692255	533.753653	9.314765
7.623752	530.876853	9.319783
7.648886	532.734863	9.324800
7.858759	533.932769	9.329818
7.707873	530.141070	9.334835
7.840545	542.967583	9.339853
7.982173	547.511868	9.344871
7.846545	539.747773	9.349888
7.712284	527.751538	9.354906
7.656768	523.089676	9.359923
7.690348	529.888348	9.364941
7.822038	536.756857	9.369959
7.907397	547.454308	9.374976
7.948707	547.785532	9.379994
7.882305	541.134058	9.385011
7.260402	527.469067	9.390029
7.742277	535.642859	9.395047
7.616057	545.025931	9.400064
7.997793	538.995364	9.405082
8.001739	547.480730	9.410099
7.880585	548.228728	9.415117
8.063109	539.695262	9.420135
8.164014	543.917723	9.425152
8.130479	535.749471	9.430170
7.831685	529.592003	9.435187
7.746221	534.951349	9.440205
7.893306	540.996939	9.445223
7.730920	542.439363	9.450240
8.027112	537.750793	9.455258
7.781022	544.987766	9.460275
7.646966	553.346433	9.465293
8.209498	539.344376	9.470311
7.766525	544.343173	9.475328
7.637798	541.400067	9.480346
7.822354	544.429151	9.485363
8.297480	540.416289	9.490381
8.385693	538.985537	9.495399
8.230988	557.600651	9.500416
8.406067	540.197380	9.505434
8.169156	543.418731	9.510451
7.957312	538.674061	9.515469
7.752103	525.369818	9.520487
7.991511	535.355160	9.525504
8.071505	540.515014	9.530522
8.097758	534.139359	9.535539
7.731880	545.920522	9.540557
7.946654	546.306618	9.545575
8.107554	540.137082	9.550592
8.273812	545.725234	9.555610
8.482856	545.159175	9.560627
7.910934	532.562479	9.565645
8.338581	541.098220	9.570663
7.755405	532.388083	9.575680
7.989895	540.221941	9.580698
7.927705	545.268374	9.585715
7.855704	550.884391	9.590733
8.082201	540.027674	9.595751
8.023494	542.602566	9.600768
8.063771	540.718578	9.605786
8.384676	541.829659	9.610803
7.915510	549.123675	9.615821
7.926110	549.011587	9.620839
7.644943	547.203208	9.625856
7.717356	550.612781	9.630874
7.866290	544.400937	9.635891
8.034925	552.513363	9.640909
8.511320	562.875000	9.645927
8.084685	570.730406	9.650944
8.010950	564.401965	9.655962
8.410762	561.394978	9.660979
8.456160	571.101469	9.665997
8.378762	552.191398	9.671015
8.099230	556.744869	9.676032
8.404486	549.126287	9.681050
8.121734	549.842801	9.686067
7.957630	550.654334	9.691085
8.381558	560.206836	9.696103
8.139390	564.094890	9.701120
8.339348	567.143655	9.706138
8.400861	571.804640	9.711155
8.492959	568.596556	9.716173
8.540072	547.902884	9.721191
7.952993	550.207114	9.726208
7.842378	545.503385	9.731226
8.339239	552.393581	9.736243
8.276734	570.697617	9.741261
8.307936	565.129062	9.746279
8.242332	574.862415	9.751296
8.251882	574.494870	9.756314
8.687584	575.483825	9.761331
8.563386	566.692290	9.766349
8.773820	563.774936	9.771367
8.317433	554.284372	9.776384
8.330761	550.429070	9.781402
8.089024	541.040582	9.786419
8.321615	553.955589	9.791437
8.190770	555.462500	9.796455
8.381979	568.731141	9.801472
8.579048	561.290451	9.806490
8.471280	569.730215	9.811507
8.603455	572.846405	9.816525
8.473192	563.342609	9.821543
8.584967	569.157056	9.826560
8.543649	572.915812	9.831578
8.618485	555.641842	9.836595
8.250248	544.095665	9.841613
8.308044	545.487812	9.846631
8.308358	567.231297	9.851648
8.732868	574.549404	9.856666
8.737144	568.675798	9.861683
8.483176	554.422962	9.866701
8.548331	546.662120	9.871719
8.492112	554.749816	9.876736
8.612045	553.882139	9.881754
8.367727	552.222620	9.886771
8.648125	555.577516	9.891789
8.782144	549.440591	9.896807
8.580833	548.888334	9.901824
8.514877	550.334585	9.906842
8.748227	540.972645	9.911859
8.454871	541.918038	9.916877
8.643029	550.159948	9.921895
8.391675	548.230133	9.926912
8.619169	545.439496	9.931930
8.765191	542.910934	9.936947
8.488504	549.906549	9.941965
8.785867	540.951146	9.946983
8.693808	549.224337	9.952000
8.286318	550.253885	9.957018
8.412838	558.688492	9.962035
8.557131	563.469049	9.967053
8.658878	568.578165	9.972071
8.741314	567.997229	9.977088
9.093833	571.385009	9.982106
9.085477	564.875910	9.987123
8.768232	553.877160	9.992141
8.820689	543.685182	9.997159
8.765633	548.806238	10.002176
8.570780	548.180385	10.007194
8.586355	537.047448	10.012211
8.818668	542.173970	10.017229
8.422758	538.023028	10.022247
8.664402	546.963456	10.027264
8.495602	559.092446	10.032282
8.851457	568.223273	10.037299
9.072693	571.101447	10.042317
9.167374	558.233031	10.047335
8.947748	551.069072	10.052352
8.634118	546.113130	10.057370
9.051774	544.236285	10.062387
8.830119	549.052084	10.067405
8.939102	549.748246	10.072423
8.874898	549.830914	10.077440
8.658654	544.468394	10.082458
8.944909	541.460268	10.087475
8.552716	543.790766	10.092493
8.672111	540.572099	10.097511
8.638284	543.477609	10.102528
8.561856	541.037549	10.107546
9.135037	558.617124	10.112563
8.688274	556.421279	10.117581
8.987246	538.897611	10.122599
8.687074	548.980127	10.127616
9.055437	567.986668	10.132634
8.838186	559.285456	10.137651
8.919907	577.046192	10.142669
9.135817	571.524435	10.147687
8.821764	564.201697	10.152704
8.656830	566.029531	10.157722
8.774582	569.738117	10.162739
8.646159	574.533004	10.167757
8.699928	569.854007	10.172775
8.631469	569.883693	10.177792
8.537994	569.642744	10.182810
9.041737	562.772542	10.187827
8.609287	569.196122	10.192845
8.544561	569.253626	10.197863
8.813646	580.250515	10.202880
8.892322	598.535615	10.207898
9.319455	596.758265	10.212915
9.180788	598.067589	10.217933
9.312925	591.627986	10.222951
9.207012	578.589012	10.227968
9.125192	581.795538	10.232986
9.038668	570.650175	10.238003
9.021019	576.516460	10.243021
9.108714	574.195848	10.248039
9.037064	570.120326	10.253056
8.905343	572.305875	10.258074
9.545349	567.547649	10.263091
9.046147	573.473605	10.268109
9.045860	581.435785	10.273127
9.030259	577.641814	10.278144
8.512239	576.040957	10.283162
9.382023	587.789489	10.288179
9.510575	596.226952	10.293197
8.997885	585.675372	10.298215
9.006393	580.757310	10.303232
9.160629	601.400588	10.308250
9.107056	596.063058	10.313267
9.337075	598.286607	10.318285
8.998453	600.501421	10.323303
9.402614	606.992750	10.328320
9.271311	598.710399	10.333338
9.124962	607.891529	10.338355
9.115177	608.091904	10.343373
9.130086	601.503407	10.348391
9.457743	604.740454	10.353408
9.255116	605.106744	10.358426
9.104086	598.604208	10.363443
9.194209	605.769591	10.368461
9.031319	602.866542	10.373479
9.280647	593.227516	10.378496
9.065250	600.724790	10.383514
9.560163	598.886327	10.388531
9.285773	597.218893	10.393549
9.106935	597.742402	10.398567
9.307703	604.524374	10.403584
9.242317	611.038781	10.408602
9.517432	596.706170	10.413619
9.104699	599.655277	10.418637
9.143168	601.173533	10.423655
9.519251	593.610108	10.428672
9.275533	597.384802	10.433690
9.540387	588.163070	10.438707
9.621795	599.486022	10.443725
9.154092	598.925008	10.448743
9.295483	592.386125	10.453760
9.333803	594.630241	10.458778
9.631513	593.974549	10.463795
9.489310	589.938480	10.468813
9.301886	599.927618	10.473831
9.273697	593.481577	10.478848
9.146460	598.045910	10.483866
9.389940	591.326929	10.488883
9.218749	602.885121	10.493901
9.082471	608.192489	10.498919
9.835301	616.462721	10.503936
9.619538	611.848034	10.508954
9.722068	602.118394	10.513971
9.364108	595.272739	10.518989
9.436278	604.309177	10.524007
9.664295	599.833245	10.529024
9.801153	602.361726	10.534042
9.726112	598.861087	10.539059
9.693131	594.078910	10.544077
9.247210	605.607565	10.549095
9.402473	591.662967	10.554112
9.549846	599.276971	10.559130
9.311210	594.170409	10.564147
9.600191	609.260445	10.569165
9.534576	613.234456	10.574183
9.610959	617.697463	10.579200
9.518619	622.679214	10.584218
9.347181	630.876516	10.589235
9.623764	627.737347	10.594253
9.240992	628.131862	10.599271
9.436121	630.780606	10.604288
9.681085	628.801421	10.609306
9.688765	631.318587	10.614323
9.987479	627.156621	10.619341
9.825327	633.692508	10.624359
10.042747	619.801266	10.629376
9.579621	627.851764	10.634394
9.697751	624.169375	10.639411
9.461131	619.526395	10.644429
9.352902	626.530360	10.649447
9.517187	624.295572	10.654464
9.629354	624.189660	10.659482
9.430823	625.353731	10.664499
10.019905	622.481182	10.669517
9.524540	624.584857	10.674535
10.008627	617.001344	10.679552
9.666644	624.436410	10.684570
9.620410	622.401865	10.689587
9.684976	624.597691	10.694605
9.377045	626.220717	10.699623
9.835703	632.034483	10.704640
9.998296	651.164872	10.709658
10.069841	640.045192	10.714675
10.080878	642.482938	10.719693
9.742374	632.901279	10.724711
9.912203	632.634853	10.729728
10.119190	624.198500	10.734746
9.849641	629.542535	10.739763
9.892035	623.211656	10.744781
9.513947	628.149817	10.749799
9.785158	628.261984	10.754816
9.906918	644.504877	10.759834
10.026386	651.419527	10.764851
10.144513	643.675590	10.769869
10.206314	636.846202	10.774887
9.714665	621.668027	10.779904
9.727546	631.550059	10.784922
10.114596	641.657497	10.789939
10.148379	639.916527	10.794957
9.747923	645.710269	10.799975
10.038422	640.426114	10.804992
10.137194	651.484445	10.810010
10.169261	643.331112	10.815027
10.120595	644.231860	10.820045
10.017929	634.543820	10.825063
10.076177	619.834913	10.830080
10.130125	620.577570	10.835098
9.996461	615.732267	10.840115
10.048290	623.922987	10.845133
9.837671	641.341426	10.850151
10.016338	640.524502	10.855168
10.329009	642.700393	10.860186
10.113363	636.779170	10.865203
10.489978	649.990420	10.870221
10.245958	638.740302	10.875239
10.187889	628.906421	10.880256
10.207694	629.007486	10.885274
10.127800	626.861448	10.890291
10.006283	626.192545	10.895309
10.092215	631.465104	10.900327
10.010290	629.101633	10.905344
10.282045	643.537986	10.910362
10.271070	650.400490	10.915379
10.428689	648.012107	10.920397
9.902129	642.291077	10.925415
10.113063	648.866346	10.930432
10.317051	650.708969	10.935450
10.368662	647.990056	10.940467
10.289924	642.034758	10.945485
10.593646	650.763538	10.950503
10.185074	641.533682	10.955520
10.221306	624.193109	10.960538
9.780820	636.408901	10.965555
10.146447	634.776885	10.970573
10.148356	649.905622	10.975591
10.330004	651.262593	10.980608
10.463511	655.786087	10.985626
10.328639	652.499940	10.990643
10.509073	647.507585	10.995661
10.295097	657.939576	11.000679
10.443845	648.464603	11.005696
10.514505	651.530485	11.010714
10.487941	648.470368	11.015731
10.502342	639.256291	11.020749
10.298784	657.749775	11.025767
10.454025	647.917177	11.030784
10.519039	658.422221	11.035802
10.715227	641.829746	11.040819
10.898578	642.350157	11.045837
10.031305	628.998090	11.050855
10.051008	630.585561	11.055872
10.494642	636.054542	11.060890
10.674252	644.698624	11.065907
10.557472	640.548106	11.070925
10.331808	648.883301	11.075943
10.646274	649.181196	11.080960
10.698795	639.292113	11.085978
10.622489	640.459125	11.090995
10.336105	616.753323	11.096013
10.439552	630.878364	11.101031
10.655338	640.378314	11.106048
10.907845	650.074489	11.111066
10.571443	626.651067	11.116083
10.393508	615.090807	11.121101
10.337310	627.416797	11.126119
10.474628	638.446990	11.131136
10.637448	641.924466	11.136154
10.638512	649.539325	11.141171
10.674645	633.252804	11.146189
10.390735	642.916256	11.151207
10.513356	646.305357	11.156224
10.618532	651.836841	11.161242
10.371582	647.943402	11.166259
10.732306	649.483756	11.171277
10.712693	649.004013	11.176295
10.657900	647.175934	11.181312
10.519299	645.995307	11.186330
10.474276	643.035914	11.191347
10.559139	640.813568	11.196365
10.316791	650.407395	11.201383
10.678957	654.200781	11.206400
10.524249	651.413207	11.211418
10.562763	654.982746	11.216435
10.832633	641.938497	11.221453
10.533071	663.211529	11.226471
10.744683	671.213133	11.231488
11.007784	675.347095	11.236506
10.376817	673.154850	11.241523
10.811277	670.215001	11.246541
10.676492	675.102430	11.251559
10.685023	670.351599	11.256576
10.876922	670.473037	11.261594
10.869520	669.546409	11.266611
10.951919	661.763880	11.271629
10.659366	670.302071	11.276647
10.926879	670.963932	11.281664
10.968080	675.151596	11.286682
10.558995	671.441348	11.291699
10.930059	666.002550	11.296717
10.727608	673.078101	11.301735
10.463811	673.551807	11.306752
10.604935	679.753014	11.311770
10.366493	678.322938	11.316787
10.687363	690.002907	11.321805
11.306242	691.546998	11.326823
10.913175	700.539612	11.331840
11.014654	689.487796	11.336858
10.899142	693.933550	11.341875
11.155811	697.017633	11.346893
11.217694	696.231628	11.351911
11.209534	695.964687	11.356928
11.240033	681.099129	11.361946
10.921482	679.984565	11.366963
10.844133	671.677947	11.371981
10.850172	684.969375	11.376999
11.237145	698.018090	11.382016
11.416367	701.016477	11.387034
11.253163	696.169469	11.392051
11.363651	671.167483	11.397069
11.054639	671.951232	11.402087
11.304460	680.170917	11.407104
11.437542	675.911813	11.412122
11.333910	679.715070	11.417139
11.132275	671.456328	11.422157
11.088738	667.022926	11.427175
11.523002	674.323767	11.432192
11.289150	674.417237	11.437210
11.054136	678.758634	11.442227
11.009009	671.510482	11.447245
11.127662	676.844200	11.452263
10.900717	674.254135	11.457280
11.319537	670.915946	11.462298
10.983567	671.031728	11.467315
11.285536	667.427824	11.472333
11.288833	672.716499	11.477351
11.246565	670.883300	11.482368
11.479098	672.150248	11.487386
10.939796	682.702654	11.492403
11.068050	658.344847	11.497421
11.216435	684.915778	11.502439
11.183252	692.097361	11.507456
11.361967	695.682811	11.512474
11.174463	698.763904	11.517491
11.429585	697.022964	11.522509
11.488463	692.614535	11.527527
11.281660	694.262748	11.532544
11.653953	686.583112	11.537562
11.696264	690.051077	11.542579
11.386968	682.837998	11.547597
11.406187	681.970315	11.552615
11.227089	692.428420	11.557632
11.564238	691.460429	11.562650
11.450706	696.653806	11.567667
11.449923	695.331661	11.572685
11.524541	693.480145	11.577703
11.551005	698.885119	11.582720
11.785522	689.336726	11.587738
11.716227	685.257653	11.592755
11.296208	674.085581	11.597773
11.564190	665.677522	11.602791
11.248576	664.893860	11.607808
11.612650	690.348557	11.612826
11.433945	698.092589	11.617843
11.446463	688.793575	11.622861
11.925874	689.286535	11.627879
11.640301	695.636655	11.632896
11.566555	684.404011	11.637914
11.453571	681.010287	11.642931
11.624539	684.035212	11.647949
11.838722	683.900693	11.652967
11.781891	692.569220	11.657984
11.978762	671.829849	11.663002
11.573438	677.933636	11.668019
11.446003	666.835648	11.673037
11.445486	674.829464	11.678055
11.649286	685.827179	11.683072
11.615983	687.681739	11.688090
11.838010	687.700626	11.693107
11.700181	694.179076	11.698125
11.563160	686.626577	11.703143
11.550481	708.028283	11.708160
11.607047	699.681735	11.713178
11.473591	697.843886	11.718195
11.430772	693.684923	11.723213
11.483090	691.051099	11.728231
11.589930	691.327877	11.733248
11.588555	687.124552	11.738266
11.471069	687.808865	11.743283
11.471682	695.682592	11.748301
11.877155	706.626631	11.753319
12.157939	722.062032	11.758336
12.197392	713.907509	11.763354
11.951853	705.475748	11.768371
11.897075	694.410541	11.773389
12.003102	688.820757	11.778407
11.534790	684.971461	11.783424
11.639326	683.433998	11.788442
12.030739	697.880049	11.793459
12.293797	708.953702	11.798477
12.104581	683.563151	11.803495
11.800318	687.262143	11.808512
11.842196	684.958163	11.813530
11.671042	696.652110	11.818547
11.437402	696.534107	11.823565
11.673841	703.474632	11.828583
11.876802	700.738308	11.833600
12.026422	709.642743	11.838618
11.898243	717.157958	11.843635
12.300243	716.211364	11.848653
12.191995	713.189281	11.853671
11.860678	723.046398	11.858688
11.871865	709.345191	11.863706
11.703494	720.609524	11.868723
11.868459	722.369906	11.873741
12.334853	713.151246	11.878759
12.324933	724.324483	11.883776
12.281680	719.322974	11.888794
12.250520	720.959448	11.893811
12.185859	719.385375	11.898829
12.216259	714.564833	11.903847
11.797941	720.752721	11.908864
12.183260	714.636326	11.913882
11.985105	722.964090	11.918899
12.169558	722.565983	11.923917
12.300530	718.891029	11.928935
11.723294	719.896689	11.933952
12.090721	719.810743	11.938970
12.485315	734.960077	11.943987
12.478132	734.879176	11.949005
12.353594	718.630375	11.954023
12.182352	719.152697	11.959040
12.077309	716.571928	11.964058
11.945568	722.219450	11.969075
12.146679	745.661089	11.974093
12.645932	743.935542	11.979111
12.541784	739.350672	11.984128
12.619586	736.053279	11.989146
12.420791	725.537642	11.994163
12.284359	718.518374	11.999181
12.360047	711.743586	12.004199
12.101052	724.230806	12.009216
12.275900	732.982975	12.014234
12.398853	751.980825	12.019251
12.708728	738.349564	12.024269
12.748671	732.637575	12.029287
12.362359	725.973038	12.034304
12.497769	714.919046	12.039322
12.211802	719.486188	12.044339
12.535111	730.575661	12.049357
12.982551	734.008561	12.054375
12.399898	734.286071	12.059392
12.354137	712.464347	12.064410
12.805440	715.663106	12.069427
12.322779	716.534026	12.074445
12.265959	710.408011	12.079463
12.429869	727.124062	12.084480
12.647676	742.433648	12.089498
12.796544	733.362558	12.094515
12.826153	731.836830	12.099533
13.048735	725.395632	12.104551
12.469734	719.865831	12.109568
12.434516	706.285507	12.114586
12.504864	707.836648	12.119603
12.605947	721.769625	12.124621
12.705062	713.735144	12.129639
12.286781	736.115626	12.134656
12.516359	735.161332	12.139674
12.900510	735.451466	12.144691
12.581352	740.254191	12.149709
13.158274	741.385134	12.154727
12.864730	746.546768	12.159744
13.018191	744.130622	12.164762
12.746076	712.643314	12.169779
12.229815	714.141197	12.174797
12.918874	729.888180	12.179815
12.664794	737.681909	12.184832
12.721478	738.304221	12.189850
12.975558	742.931923	12.194867
12.592428	733.754837	12.199885
12.768417	730.378945	12.204903
12.794179	743.184483	12.209920
12.894198	735.269772	12.214938
12.957439	742.900175	12.219955
12.323830	744.479563	12.224973
12.943938	734.801302	12.229991
12.934458	746.593029	12.235008
12.862303	739.885577	12.240026
12.891184	743.668084	12.245043
12.627152	743.109869	12.250061
12.812655	738.044110	12.255079
12.859080	738.207277	12.260096
12.955487	734.947995	12.265114
13.102696	737.544301	12.270131
12.767274	739.553501	12.275149
13.371679	742.873446	12.280167
12.931462	734.844562	12.285184
12.919640	740.403872	12.290202
12.638252	738.592352	12.295219
12.634330	740.767365	12.300237
13.110687	746.947629	12.305255
12.892875	760.763342	12.310272
13.067587	767.006654	12.315290
13.258015	761.940117	12.320307
13.015872	775.185289	12.325325
13.361802	770.574074	12.330343
13.362530	775.437143	12.335360
13.387251	769.986306	12.340378
13.622346	750.294908	12.345395
13.243140	750.606815	12.350413
13.205354	743.875041	12.355431
13.353502	740.096405	12.360448
13.239328	735.440522	12.365466
13.461503	738.804575	12.370483
12.991345	740.995833	12.375501
12.931148	739.484176	12.380519
13.085158	737.254140	12.385536
12.948886	750.678368	12.390554
13.356398	761.189771	12.395571
12.989049	769.468326	12.400589
13.619652	762.136354	12.405607
13.612816	769.067683	12.410624
13.394541	763.260441	12.415642
13.653599	756.008777	12.420659
13.128968	751.335148	12.425677
13.400945	752.494935	12.430695
13.369520	746.740475	12.435712
13.371223	760.139937	12.440730
13.119863	747.294044	12.445747
13.549233	761.396525	12.450765
13.511755	761.967318	12.455783
13.594192	766.741842	12.460800
13.508341	766.446046	12.465818
13.647696	759.920044	12.470835
13.340267	751.965022	12.475853
13.067192	745.087074	12.480871
13.533772	761.405436	12.485888
13.523091	761.470252	12.490906
13.682688	763.266193	12.495923
13.270337	762.437722	12.500941
13.562308	763.423962	12.505959
13.605030	765.427566	12.510976
13.526365	756.540440	12.515994
14.003183	763.730507	12.521011
13.489193	760.036677	12.526029
13.594814	764.678178	12.531047
13.679519	764.702802	12.536064
13.557956	766.047328	12.541082
13.779953	756.068509	12.546099
13.456585	767.574911	12.551117
13.738869	766.959500	12.556135
13.653285	768.484584	12.561152
13.444022	768.627851	12.566170
13.844913	751.280514	12.571187
13.901678	763.301716	12.576205
13.689651	761.908521	12.581223
13.765360	766.867138	12.586240
13.659810	760.802390	12.591258
13.822086	765.160457	12.596275
13.449200	771.025659	12.601293
13.766572	760.599544	12.606311
13.816914	761.276500	12.611328
13.666195	761.637815	12.616346
13.896876	758.695166	12.621363
13.852780	768.649319	12.626381
13.436337	759.950815	12.631399
13.953497	762.018941	12.636416
13.662962	768.439292	12.641434
13.785865	756.926479	12.646451
13.456927	763.090910	12.651469
13.959934	778.696673	12.656487
14.310140	779.878919	12.661504
13.944734	777.206390	12.666522
14.003912	766.205335	12.671539
14.043384	765.290293	12.676557
13.510109	760.349770	12.681575
13.931554	771.038879	12.686592
14.231052	775.810954	12.691610
14.625847	773.230758	12.696627
14.236472	771.612881	12.701645
14.400756	762.110167	12.706663
14.179677	756.341237	12.711680
14.077937	753.788347	12.716698
14.132349	760.454454	12.721715
13.628829	762.363760	12.726733
13.790746	759.091054	12.731751
14.300604	762.921284	12.736768
14.114530	770.843229	12.741786
14.077894	768.018202	12.746803
13.948715	781.384537	12.751821
14.184435	779.065953	12.756839
14.351853	783.631504	12.761856
14.422659	784.267384	12.766874
14.396043	779.383173	12.771891
14.210044	775.382326	12.776909
14.340149	764.878251	12.781927
14.218251	770.104518	12.786944
14.189725	769.897571	12.791962
14.480582	772.900571	12.796979
14.148523	770.961285	12.801997
14.421312	765.361128	12.807015
14.272896	773.103603	12.812032
14.110681	780.614710	12.817050
14.424410	771.483057	12.822067
14.310628	768.180961	12.827085
14.445582	774.739778	12.832103
14.478660	774.838764	12.837120
14.203353	778.201874	12.842138
14.504560	775.061978	12.847155
14.160668	774.099702	12.852173
14.409553	773.921875	12.857191
14.659753	775.612102	12.862208
14.209927	774.379242	12.867226
14.452300	781.019062	12.872243
14.767032	784.652648	12.877261
14.580073	777.003792	12.882279
14.656530	776.613137	12.887296
14.424266	782.083921	12.892314
14.758241	780.838709	12.897331
14.348280	782.717579	12.902349
14.287612	782.146434	12.907367
14.492037	776.702153	12.912384
14.805591	774.342972	12.917402
14.821211	774.681381	12.922419
14.575151	786.336630	12.927437
14.435567	780.908378	12.932455
14.796140	778.485024	12.937472
14.382860	786.575120	12.942490
14.417953	786.926258	12.947507
14.530313	780.874699	12.952525
14.669854	777.829561	12.957543
14.461041	774.501327	12.962560
14.323100	771.783692	12.967578
14.533819	795.921334	12.972595
14.490639	807.039873	12.977613
14.790501	810.230819	12.982631
15.086528	804.822672	12.987648
14.866378	817.745689	12.992666
15.109534	799.274289	12.997683
14.900496	805.599832	13.002701
14.911040	808.810862	13.007719
14.919434	798.982253	13.012736
14.883929	806.738610	13.017754
14.896416	803.281022	13.022771
15.103998	805.438684	13.027789
14.921329	804.836160	13.032807
15.193763	803.158770	13.037824
15.188213	792.748517	13.042842
14.694090	774.146504	13.047859
15.052379	774.150354	13.052877
14.736913	785.475645	13.057895
15.333297	789.866688	13.062912
14.968271	780.863469	13.067930
15.196536	779.972495	13.072947
14.981918	774.767443	13.077965
15.137686	768.810074	13.082983
15.255658	773.585344	13.088000
15.010492	769.536962	13.093018
15.051351	764.777885	13.098035
15.211467	772.175369	13.103053
15.118938	769.179216	13.108071
15.084703	767.546722	13.113088
15.022055	784.636000	13.118106
14.914124	786.543288	13.123123
15.422247	790.638888	13.128141
15.477768	789.307914	13.133159
15.451522	771.266921	13.138176
15.417009	765.052185	13.143194
15.220763	759.708558	13.148211
15.650978	756.289672	13.153229
15.178770	762.568070	13.158247
15.511655	762.863081	13.163264
15.220574	767.159635	13.168282
15.284398	760.355129	13.173299
15.129656	758.911933	13.178317
14.924106	762.330383	13.183335
15.345532	757.006745	13.188352
15.045936	777.263737	13.193370
15.294735	781.115939	13.198387
15.758567	781.961642	13.203405
15.714973	789.198544	13.208423
15.606392	772.710505	13.213440
15.666121	768.529145	13.218458
15.507618	772.896447	13.223475
15.573195	762.585522	13.228493
15.624419	764.496275	13.233511
15.468112	768.538180	13.238528
15.251224	765.302733	13.243546
15.231765	766.441911	13.248563
15.150985	771.844775	13.253581
15.455894	779.071251	13.258599
15.770099	782.263101	13.263616
15.572581	789.950159	13.268634
15.719297	794.607321	13.273651
15.888276	791.342970	13.278669
15.478554	789.100265	13.283687
15.791478	775.373822	13.288704
15.549329	784.342832	13.293722
15.726763	793.495419	13.298739
15.831991	787.366079	13.303757
15.345286	786.034854	13.308775
15.562019	782.949217	13.313792
15.434053	791.531107	13.318810
15.494087	797.656696	13.323827
15.737660	786.058686	13.328845
15.845778	788.708462	13.333863
16.012840	790.134002	13.338880
15.649804	789.136855	13.343898
15.825979	791.173202	13.348915
15.877913	793.162742	13.353933
15.792738	799.434162	13.358951
15.937785	788.164016	13.363968
15.731312	787.003482	13.368986
15.693932	782.026281	13.374003
15.979572	774.489574	13.379021
15.699813	787.182065	13.384039
15.958488	786.052793	13.389056
15.869578	794.013175	13.394074
15.603433	790.608713	13.399091
16.095394	777.368620	13.404109
15.628123	797.746581	13.409127
15.927095	799.722663	13.414144
15.832851	809.362799	13.419162
15.673230	815.109394	13.424179
16.091861	811.099013	13.429197
15.943773	810.904487	13.434215
16.183459	806.010103	13.439232
16.005519	811.361929	13.444250
16.137502	812.089212	13.449267
16.276843	813.730540	13.454285
15.543734	810.071030	13.459303
16.029985	809.963311	13.464320
16.372053	810.089624	13.469338
16.204668	811.668555	13.474355
15.892555	806.866938	13.479373
16.018715	813.247264	13.484391
16.543618	806.051758	13.489408
15.980916	816.282855	13.494426
16.249429	810.891641	13.499443
16.585219	814.155855	13.504461
15.953773	816.953069	13.509479
16.214312	810.597413	13.514496
15.964472	810.759662	13.519514
16.073426	814.946211	13.524531
16.437642	821.939347	13.529549
16.457298	831.116673	13.534567
16.890868	828.271614	13.539584
16.331570	817.137054	13.544602
16.146701	817.506877	13.549619
15.970756	814.157707	13.554637
16.221563	834.117083	13.559655
16.644706	832.002660	13.564672
16.496351	833.196752	13.569690
16.449840	838.348111	13.574707
16.391973	832.815519	13.579725
16.613937	841.961154	13.584743
16.727201	836.673152	13.589760
16.618987	841.285060	13.594778
16.509640	831.039373	13.599795
16.565493	833.754151	13.604813
16.656899	841.998731	13.609831
16.518817	839.344224	13.614848
16.556418	843.456752	13.619866
16.505378	839.469459	13.624883
16.743401	840.044427	13.629901
16.548209	845.219083	13.634919
16.901602	836.825964	13.639936
17.071975	835.271861	13.644954
17.020100	840.446151	13.649971
17.074843	832.109295	13.654989
16.912151	831.793979	13.660007
16.634676	824.074076	13.665024
16.671721	811.744691	13.670042
16.871393	830.582280	13.675059
17.112845	824.299039	13.680077
16.769135	832.596009	13.685095
16.949435	825.315631	13.690112
16.904703	817.489836	13.695130
16.688016	817.274499	13.700147
16.891444	822.819045	13.705165
16.878745	827.135112	13.710183
16.732685	837.225202	13.715200
16.726270	834.752041	13.720218
16.696758	845.720137	13.725235
17.291485	833.101385	13.730253
16.877712	832.746512	13.735271
17.021487	835.580060	13.740288
17.209277	838.580284	13.745306
16.854825	841.387753	13.750323
17.134571	826.804919	13.755341
17.027669	839.495611	13.760359
17.157518	833.791594	13.765376
17.170393	829.557600	13.770394
16.965976	830.489072	13.775411
17.272438	834.616278	13.780429
17.027078	838.015733	13.785447
17.082598	832.405415	13.790464
17.138582	840.639766	13.795482
16.812781	833.669057	13.800499
16.928017	827.004796	13.805517
17.053905	834.360331	13.810535
17.222035	827.444782	13.815552
17.317335	824.905192	13.820570
16.428963	832.927733	13.825587
17.179481	836.887533	13.830605
17.259607	857.631084	13.835623
17.398082	849.659803	13.840640
17.453992	861.252009	13.845658
17.495479	863.157985	13.850675
17.252115	859.140860	13.855693
17.529089	857.595300	13.860711
17.477322	852.705542	13.865728
17.473478	856.436396	13.870746
17.397912	855.905453	13.875763
17.685152	854.806416	13.880781
17.573713	855.379333	13.885799
17.639440	846.052965	13.890816
17.222967	847.670926	13.895834
17.691825	851.103649	13.900851
17.531985	848.509356	13.905869
17.510753	847.840510	13.910887
17.422966	844.351287	13.915904
17.651546	851.826442	13.920922
17.630239	860.085534	13.925939
17.420503	854.529393	13.930957
17.551865	858.643013	13.935975
17.510200	854.528014	13.940992
17.720145	856.461245	13.946010
17.332394	868.280761	13.951027
17.487459	854.957694	13.956045
17.387436	857.529637	13.961063
17.604096	860.159262	13.966080
17.636936	854.956441	13.971098
17.376050	855.369733	13.976115
17.374402	858.134550	13.981133
17.773436	874.274248	13.986151
17.474330	879.629300	13.991168
17.838316	875.955676	13.996186
17.769443	884.086530	14.001203
17.641924	878.927762	14.006221
17.828385	886.513674	14.011239
17.739023	880.821897	14.016256
18.184223	876.343427	14.021274
18.009416	884.629737	14.026291
18.043005	881.995665	14.031309
18.206010	883.832110	14.036327
18.300905	881.462993	14.041344
18.421663	878.528080	14.046362
18.422066	888.106091	14.051379
18.142326	872.067663	14.056397
18.084901	850.023531	14.061415
18.143727	847.650602	14.066432
17.985104	845.188664	14.071450
17.980920	853.451383	14.076467
18.074288	857.132291	14.081485
18.238189	871.734053	14.086503
18.108221	869.759937	14.091520
18.463926	865.099828	14.096538
18.249987	865.164932	14.101555
18.429614	857.092525	14.106573
18.156741	846.156070	14.111591
18.262189	850.936479	14.116608
18.400259	843.561722	14.121626
18.246589	851.743718	14.126643
18.318655	845.581684	14.131661
18.494762	846.690226	14.136679
18.170532	846.633752	14.141696
18.494321	844.793675	14.146714
18.287421	847.480194	14.151731
17.858260	844.931254	14.156749
18.098735	845.957126	14.161767
18.163788	869.660091	14.166784
18.031028	865.565674	14.171802
18.258710	869.058279	14.176819
18.349714	865.477922	14.181837
18.568161	874.169680	14.186855
18.505934	874.788537	14.191872
18.590294	862.019351	14.196890
18.486681	874.125717	14.201907
18.552950	876.987195	14.206925
18.495094	866.294755	14.211943
18.402009	866.763809	14.216960
18.356384	864.148462	14.221978
18.331472	870.625063	14.226995
18.599758	868.478094	14.232013
18.465074	867.801776	14.237031
18.454147	878.419836	14.242048
18.872804	889.141011	14.247066
18.999342	892.841977	14.252083
18.903605	882.559413	14.257101
18.619898	873.167858	14.262119
18.805807	865.804531	14.267136
18.995504	872.272755	14.272154
18.557048	872.467712	14.277171
18.696146	869.675096	14.282189
19.018336	885.378712	14.287207
18.882307	881.824456	14.292224
19.065343	873.571622	14.297242
18.788640	868.366802	14.302259
18.909378	858.410104	14.307277
18.869303	864.387297	14.312295
18.959093	888.496673	14.317312
19.233776	887.042990	14.322330
18.945419	873.678929	14.327347
18.743908	860.231841	14.332365
18.787648	870.049210	14.337383
18.957154	881.150251	14.342400
19.060560	883.807092	14.347418
19.147811	896.296987	14.352435
18.926217	884.055413	14.357453
19.310705	885.838222	14.362471
19.271224	890.840169	14.367488
19.246419	888.328856	14.372506
18.851959	889.798201	14.377523
18.987084	895.593316	14.382541
19.445238	891.756610	14.387559
19.435951	886.036506	14.392576
19.404398	886.316035	14.397594
19.256479	884.707654	14.402611
19.269720	891.515963	14.407629
19.468115	883.371174	14.412647
19.362685	896.112168	14.417664
19.251480	888.079003	14.422682
19.542111	891.978324	14.427699
19.519511	881.845252	14.432717
19.315257	868.531134	14.437735
19.369130	877.990307	14.442752
19.468510	879.710487	14.447770
19.558936	872.576717	14.452787
18.674494	874.217507	14.457805
19.427612	875.778453	14.462823
19.331088	888.477021	14.467840
19.923817	884.578204	14.472858
19.760150	883.638178	14.477875
19.742609	887.790914	14.482893
19.608751	889.099506	14.487911
19.730719	888.670159	14.492928
19.869505	876.012358	14.497946
19.682702	862.689199	14.502963
19.419621	862.137142	14.507981
19.526682	858.339672	14.512999
19.207729	872.985530	14.518016
19.531529	870.485873	14.523034
19.795477	885.794664	14.528051
19.608696	885.700876	14.533069
19.819853	873.868041	14.538087
19.592171	884.718886	14.543104
19.163768	893.278467	14.548122
19.596129	885.586179	14.553139
19.383680	888.661745	14.558157
19.778774	886.359203	14.563175
19.656753	884.759388	14.568192
19.297555	887.845322	14.573210
19.591519	892.570959	14.578227
20.036803	902.704135	14.583245
20.628058	903.899117	14.588263
20.267712	913.558911	14.593280
20.223165	893.586115	14.598298
19.747514	887.677143	14.603315
19.845445	892.294636	14.608333
19.784617	880.908363	14.613351
19.699025	899.999008	14.618368
20.067540	902.046258	14.623386
20.087234	907.294562	14.628403
19.824328	915.168648	14.633421
20.103467	906.944924	14.638439
20.034790	910.401919	14.643456
20.196081	905.608155	14.648474
20.044414	907.856831	14.653491
20.255202	914.100855	14.658509
20.038401	915.605484	14.663527
20.125108	910.346868	14.668544
20.271132	909.329916	14.673562
20.615444	914.189684	14.678579
20.138193	910.193413	14.683597
20.448060	905.164927	14.688615
20.466974	908.548236	14.693632
20.225812	906.970242	14.698650
20.354004	911.860715	14.703667
19.929604	908.771365	14.708685
20.515919	907.429803	14.713703
20.114794	909.594485	14.718720
20.078841	907.113319	14.723738
20.070186	912.331352	14.728755
20.373347	935.485848	14.733773
20.621956	932.451997	14.738791
20.720551	935.740774	14.743808
20.437299	930.571676	14.748826
20.492601	932.251429	14.753843
20.478520	937.404047	14.758861
20.891341	934.117244	14.763879
20.769504	934.287841	14.768896
20.746519	926.635320	14.773914
20.293577	916.834746	14.778931
20.355128	923.569224	14.783949
20.619586	924.588188	14.788967
20.340801	931.678956	14.793984
20.673069	938.790755	14.799002
20.631182	931.052829	14.804019
20.430923	930.298419	14.809037
20.742478	927.889037	14.814055
20.881476	937.713609	14.819072
20.601614	937.110529	14.824090
20.956158	930.497099	14.829107
20.740350	936.864776	14.834125
20.649589	929.472186	14.839143
20.783534	934.418570	14.844160
20.725399	929.419333	14.849178
20.826532	944.330797	14.854195
20.564893	958.658469	14.859213
20.763779	959.166988	14.864231
20.877928	958.107689	14.869248
21.042676	959.890220	14.874266
21.320774	959.960285	14.879283
20.879364	958.776586	14.884301
20.970725	948.063875	14.889319
20.703777	961.448774	14.894336
20.749596	963.041651	14.899354
20.828564	960.201636	14.904371
21.039248	949.104147	14.909389
21.272757	953.795089	14.914407
21.228781	962.436486	14.919424
21.219180	952.847303	14.924442
21.625239	959.019721	14.929459
21.017611	961.671211	14.934477
21.452250	948.146477	14.939495
21.508113	954.055018	14.944512
21.321082	952.960855	14.949530
21.600928	952.961217	14.954547
21.473063	958.551400	14.959565
21.480537	955.700496	14.964583
21.105020	958.022122	14.969600
21.331611	967.343825	14.974618
21.726683	947.753379	14.979635
21.319202	962.839225	14.984653
21.656264	950.948743	14.989671
21.609839	958.066233	14.994688
21.503164	946.535619	14.999706
21.778627	950.380524	15.004723
21.457441	951.289271	15.009741
21.440436	953.725142	15.014759
21.336345	948.158731	15.019776
21.571818	956.200907	15.024794
21.656778	946.944058	15.029811
21.703144	959.430935	15.034829
21.913850	963.276522	15.039847
21.700843	955.262432	15.044864
21.594141	951.921323	15.049882
21.533559	954.171513	15.054899
21.937411	967.542836	15.059917
21.950754	972.435541	15.064935
21.792614	972.854829	15.069952
21.896085	976.026082	15.074970
21.767958	968.225911	15.079987
22.025052	976.911664	15.085005
22.083487	966.544935	15.090023
22.027996	951.762054	15.095040
21.706999	953.147309	15.100058
22.384686	962.593997	15.105075
22.045630	956.426910	15.110093
21.856434	943.176651	15.115111
21.916905	946.506118	15.120128
21.897444	952.142431	15.125146
22.101926	956.446594	15.130163
22.036268	972.059571	15.135181
22.110054	973.376662	15.140199
22.436029	974.458575	15.145216
22.043874	978.155618	15.150234
22.260024	958.268138	15.155251
22.238135	974.540151	15.160269
22.191607	969.662163	15.165287
22.228155	956.401772	15.170304
22.414369	971.126355	15.175322
22.285012	953.795627	15.180339
21.861028	957.144195	15.185357
22.210798	968.434802	15.190375
22.038834	974.666231	15.195392
21.828724	977.340649	15.200410
21.799458	973.472994	15.205427
21.991604	975.049257	15.210445
22.096293	974.928736	15.215463
22.155341	993.734880	15.220480
22.068683	996.759197	15.225498
22.626083	999.742565	15.230515
22.567937	1003.327319	15.235533
22.580314	996.237287	15.240551
22.696909	984.936761	15.245568
22.711237	993.638467	15.250586
22.781273	989.398635	15.255603
22.602444	997.370040	15.260621
22.535485	995.461778	15.265639
22.940997	994.814430	15.270656
22.929671	1004.732021	15.275674
23.219814	988.853514	15.280691
22.868589	973.410033	15.285709
22.655489	977.568183	15.290727
22.935582	973.226014	15.295744
22.366031	971.428059	15.300762
22.478694	970.561501	15.305779
22.714375	976.476591	15.310797
22.705805	993.939457	15.315815
23.032451	995.393661	15.320832
22.970023	1006.900358	15.325850
23.068394	993.728085	15.330867
23.050207	988.896146	15.335885
22.770534	993.260395	15.340903
22.900169	991.416008	15.345920
22.790390	998.294126	15.350938
23.047104	1003.461140	15.355955
22.658408	1002.379636	15.360973
22.491777	995.589057	15.365991
23.001206	993.259120	15.371008
22.908901	1000.513207	15.376026
22.892119	993.727554	15.381043
23.289783	998.714689	15.386061
22.855474	1001.301158	15.391079
23.116963	1006.123433	15.396096
23.179426	1013.605748	15.401114
23.334121	1021.581712	15.406131
23.276534	1025.119044	15.411149
23.194675	1017.687153	15.416167
23.353955	1020.133284	15.421184
23.359573	1016.929202	15.426202
22.988987	1029.503547	15.431219
23.204840	1015.779506	15.436237
23.265634	1021.460073	15.441255
23.555608	1018.763719	15.446272
23.652214	1024.965709	15.451290
23.646109	1015.448531	15.456307
23.711264	1017.975682	15.461325
23.700719	1022.477657	15.466343
23.698229	1020.717086	15.471360
23.516561	1031.582901	15.476378
23.735754	1023.381140	15.481395
23.978334	1021.282362	15.486413
23.822711	1021.587645	15.491431
23.586161	1003.068115	15.496448
23.645664	1008.120859	15.501466
23.619647	1008.674085	15.506483
23.579307	1013.253311	15.511501
23.367011	1018.156134	15.516519
23.971325	1014.659428	15.521536
23.567920	1017.944820	15.526554
23.806382	1024.938804	15.531571
23.916168	1020.620152	15.536589
23.899269	1018.135985	15.541607
24.208332	1011.087827	15.546624
23.767661	1012.693813	15.551642
23.696262	1014.525973	15.556659
23.925292	1012.126354	15.561677
24.096875	1010.732997	15.566695
23.971515	1010.452854	15.571712
23.671154	1010.806061	15.576730
23.764391	1010.901934	15.581747
23.757431	1020.648432	15.586765
24.045162	1003.817211	15.591783
24.036682	1012.109079	15.596800
23.792479	1011.465694	15.601818
23.587119	1004.636998	15.606835
23.855350	1016.527406	15.611853
24.048115	1034.851884	15.616871
24.083483	1037.651955	15.621888
24.148397	1044.086142	15.626906
24.340323	1033.048346	15.631923
24.456905	1036.974969	15.636941
24.190771	1031.809471	15.641959
24.648615	1037.396275	15.646976
24.576180	1032.522330	15.651994
24.286453	1033.871133	15.657011
24.289347	1035.899943	15.662029
24.317262	1036.479434	15.667047
24.431677	1034.893055	15.672064
24.140762	1039.473677	15.677082
24.396047	1035.299486	15.682099
24.400373	1033.607276	15.687117
24.329152	1034.656749	15.692135
24.737671	1032.711857	15.697152
24.453720	1038.989257	15.702170
24.353499	1029.963356	15.707187
24.393460	1034.495292	15.712205
24.200882	1040.849897	15.717223
24.880656	1042.072047	15.722240
25.049985	1059.743796	15.727258
24.844610	1048.875539	15.732275
24.983534	1035.520152	15.737293
24.854258	1029.156065	15.742311
24.810087	1020.418041	15.747328
25.057132	1020.524530	15.752346
24.409543	1020.228377	15.757363
24.868380	1030.466804	15.762381
24.961143	1036.861910	15.767399
25.029346	1036.930147	15.772416
24.757160	1035.091907	15.777434
25.055224	1045.121996	15.782451
25.069743	1034.604313	15.787469
24.816004	1052.815726	15.792487
25.143984	1043.899458	15.797504
25.181591	1047.147317	15.802522
25.345690	1051.091746	15.807539
25.427618	1029.063430	15.812557
24.863373	1023.060994	15.817575
25.214797	1035.121421	15.822592
25.308478	1040.538059	15.827610
25.064274	1038.607069	15.832627
25.265415	1032.260641	15.837645
25.298292	1042.827753	15.842663
25.109821	1045.460919	15.847680
25.368347	1048.080857	15.852698
25.544266	1042.085526	15.857715
25.770129	1030.395455	15.862733
25.429232	1029.824026	15.867751
25.420823	1019.136371	15.872768
25.320234	1016.624290	15.877786
25.011735	1022.116558	15.882803
25.340781	1032.050265	15.887821
25.223568	1048.229980	15.892839
25.490460	1046.534501	15.897856
25.402417	1056.820756	15.902874
25.370197	1050.510885	15.907891
25.479723	1050.569491	15.912909
25.319840	1044.620460	15.917927
25.450970	1051.991043	15.922944
25.361004	1049.212198	15.927962
25.317401	1055.180540	15.932979
25.459605	1052.605166	15.937997
25.526567	1052.802989	15.943015
25.854900	1068.660443	15.948032
25.858491	1068.224392	15.953050
25.904970	1063.574810	15.958067
26.086338	1062.523909	15.963085
26.142379	1061.871351	15.968103
26.535855	1054.055692	15.973120
26.108789	1045.567001	15.978138
26.001128	1040.070549	15.983155
26.222328	1029.144936	15.988173
25.859741	1035.560892	15.993191
26.097430	1029.761019	15.998208
26.241386	1030.748375	16.003226
25.872277	1027.943839	16.008243
26.144887	1028.727996	16.013261
26.124415	1028.466134	16.018279
25.779746	1020.879753	16.023296
25.969829	1021.238170	16.028314
25.943721	1033.316722	16.033331
26.059443	1023.764671	16.038349
26.257742	1036.164680	16.043367
26.347679	1050.566733	16.048384
26.309396	1052.744012	16.053402
26.348910	1044.898606	16.058419
26.349158	1047.082471	16.063437
26.361338	1059.653672	16.068455
26.441384	1049.952558	16.073472
26.037961	1060.329256	16.078490
26.762770	1063.974392	16.083507
26.907419	1053.729808	16.088525
26.689232	1051.567516	16.093543
26.452688	1042.663956	16.098560
26.550520	1038.495499	16.103578
26.803130	1044.815069	16.108595
26.738251	1037.459407	16.113613
26.250412	1036.626969	16.118631
26.736795	1043.588429	16.123648
26.605177	1048.541737	16.128666
26.787610	1053.070290	16.133683
27.073076	1047.411253	16.138701
26.602525	1035.978620	16.143719
26.739357	1044.149903	16.148736
27.008678	1047.661267	16.153754
26.927373	1038.692360	16.158771
26.648849	1022.549461	16.163789
26.194992	1033.177049	16.168807
26.647768	1038.417499	16.173824
26.982161	1044.727412	16.178842
26.653887	1054.016173	16.183859
27.055483	1051.368599	16.188877
26.716548	1047.511575	16.193895
26.749994	1048.591988	16.198912
27.073769	1039.745811	16.203930
26.495664	1046.255499	16.208947
26.668691	1047.544422	16.213965
26.886720	1053.878881	16.218983
26.693014	1063.553673	16.224000
27.248347	1064.274599	16.229018
26.996530	1071.572643	16.234035
27.158259	1066.557855	16.239053
27.395695	1064.693415	16.244071
27.333585	1071.709263	16.249088
27.351132	1071.618174	16.254106
26.855969	1074.728599	16.259123
26.955537	1066.873775	16.264141
26.907515	1074.184071	16.269159
27.156030	1085.698907	16.274176
27.042551	1098.046819	16.279194
27.221766	1095.522446	16.284211
27.495448	1092.241636	16.289229
27.453211	1092.478660	16.294247
27.556112	1090.587957	16.299264
27.705397	1088.197667	16.304282
27.617913	1099.077169	16.309299
28.085475	1091.451864	16.314317
27.840079	1094.040306	16.319335
27.759061	1096.268469	16.324352
27.937111	1087.085327	16.329370
27.709269	1091.602430	16.334387
27.511958	1095.641365	16.339405
27.840462	1085.901304	16.344423
27.624430	1087.563622	16.349440
27.759682	1077.702360	16.354458
27.743431	1088.264573	16.359475
27.948879	1081.229466	16.364493
27.933715	1089.617095	16.369511
27.614756	1089.692342	16.374528
27.862573	1083.979230	16.379546
27.546285	1090.485784	16.384563
27.648834	1090.583354	16.389581
27.900617	1106.695840	16.394599
28.244419	1112.818104	16.399616
28.182427	1116.169946	16.404634
27.945394	1117.873428	16.409651
28.185426	1115.528878	16.414669
28.042727	1107.320662	16.419687
28.264811	1118.180076	16.424704
28.283197	1111.275255	16.429722
28.316855	1112.573396	16.434739
28.376049	1113.324720	16.439757
28.283744	1106.014353	16.444775
28.430045	1111.735202	16.449792
28.446170	1108.709344	16.454810
28.045169	1117.444625	16.459827
28.312809	1113.189583	16.464845
28.665675	1114.242045	16.469863
28.242257	1117.502187	16.474880
28.550311	1119.549469	16.479898
28.242348	1112.187679	16.484915
28.227678	1106.313709	16.489933
28.461430	1118.884951	16.494951
28.561941	1112.784642	16.499968
28.802517	1124.982423	16.504986
28.371153	1127.861947	16.510003
28.597829	1131.894423	16.515021
28.885275	1136.838904	16.520039
28.932778	1144.487724	16.525056
28.752804	1131.617745	16.530074
29.018453	1136.912791	16.535091
28.977683	1139.567012	16.540109
29.096310	1131.273657	16.545127
28.748129	1120.427731	16.550144
29.335490	1114.049165	16.555162
28.684754	1112.740457	16.560179
28.531715	1112.152215	16.565197
28.786125	1129.005947	16.570215
28.723293	1135.109876	16.575232
28.929791	1129.403224	16.580250
28.994188	1137.301867	16.585267
28.861696	1137.578280	16.590285
29.134186	1139.040981	16.595303
29.167752	1135.598962	16.600320
29.249290	1123.559046	16.605338
28.757344	1136.281873	16.610355
29.069563	1130.429264	16.615373
29.217029	1140.028551	16.620391
29.053250	1139.511421	16.625408
29.025578	1146.155817	16.630426
29.155285	1152.952289	16.635443
29.410219	1153.133286	16.640461
29.366888	1150.205102	16.645479
29.128393	1166.176700	16.650496
29.429674	1157.583307	16.655514
29.697045	1161.363252	16.660531
29.859095	1159.135060	16.665549
29.650219	1151.833470	16.670567
29.425193	1163.772857	16.675584
29.275356	1160.845579	16.680602
29.459251	1157.102282	16.685619
29.517147	1158.308263	16.690637
29.903124	1153.513944	16.695655
29.677975	1164.415055	16.700672
29.475429	1153.016098	16.705690
29.554839	1160.003496	16.710707
30.019144	1171.102711	16.715725
30.281088	1175.464199	16.720743
29.700719	1166.144216	16.725760
29.978311	1164.254538	16.730778
29.981713	1167.835994	16.735795
30.046285	1169.820440	16.740813
29.980600	1163.430562	16.745831
30.011774	1175.478143	16.750848
30.262350	1173.245547	16.755866
30.458365	1170.311419	16.760883
30.645626	1148.705124	16.765901
30.209593	1154.280533	16.770919
29.996085	1153.884807	16.775936
30.048608	1144.642405	16.780954
30.488225	1157.594845	16.785971
30.376053	1150.413809	16.790989
30.304470	1147.471117	16.796007
30.261617	1147.439985	16.801024
30.201149	1144.104219	16.806042
30.338197	1148.851353	16.811059
30.446520	1157.958150	16.816077
30.428281	1149.588397	16.821095
30.371216	1155.502075	16.826112
30.427270	1163.818617	16.831130
30.578438	1165.587517	16.836147
30.328677	1169.192858	16.841165
30.254242	1166.389470	16.846183
30.415545	1175.718356	16.851200
30.533600	1166.216359	16.856218
30.537919	1170.532999	16.861235
30.367535	1173.589399	16.866253
30.588452	1168.805159	16.871271
30.501010	1170.608288	16.876288
30.636789	1170.400841	16.881306
30.861531	1175.522421	16.886323
30.704719	1181.192950	16.891341
31.098223	1181.686763	16.896359
30.784155	1176.036411	16.901376
30.657861	1184.466742	16.906394
30.961546	1197.188035	16.911411
30.777880	1186.773900	16.916429
31.085039	1189.335745	16.921447
30.798244	1199.785772	16.926464
30.908107	1201.744190	16.931482
31.300281	1188.844489	16.936499
31.381039	1190.141568	16.941517
31.351793	1192.011323	16.946535
31.342616	1198.485578	16.951552
31.392306	1183.992150	16.956570
31.413165	1196.975513	16.961587
31.128114	1190.234973	16.966605
31.307573	1191.298829	16.971623
31.318464	1192.105063	16.976640
31.468087	1184.977673	16.981658
31.832481	1185.678026	16.986675
31.362167	1187.235021	16.991693
31.571980	1182.184264	16.996711
31.386496	1188.465224	17.001728
31.880155	1187.106601	17.006746
31.398228	1193.692794	17.011763
31.175887	1201.970919	17.016781
31.914009	1182.026657	17.021799
31.890694	1189.374156	17.026816
31.759804	1188.798221	17.031834
31.659356	1186.639557	17.036851
31.305114	1193.256239	17.041869
31.678964	1194.740935	17.046887
31.397454	1191.408233	17.051904
31.915018	1185.270960	17.056922
31.847761	1182.453821	17.061939
31.738159	1186.185533	17.066957
31.993292	1188.758685	17.071975
31.699800	1190.120713	17.076992
31.808956	1198.204881	17.082010
31.987266	1212.700520	17.087027
32.008179	1215.086302	17.092045
32.021386	1211.473883	17.097063
31.555406	1210.142531	17.102080
31.868539	1211.463166	17.107098
32.178192	1213.320853	17.112115
32.351903	1206.615730	17.117133
32.422587	1198.945260	17.122151
32.246760	1205.821182	17.127168
32.680046	1206.611732	17.132186
32.598527	1203.844163	17.137203
32.376042	1202.774474	17.142221
32.606269	1206.348802	17.147239
32.755407	1212.608902	17.152256
32.255283	1213.409992	17.157274
32.597291	1201.297655	17.162291
32.661858	1211.001491	17.167309
32.464616	1199.904640	17.172327
32.518475	1206.618339	17.177344
32.314867	1207.827424	17.182362
32.583975	1210.281621	17.187379
32.559503	1207.956410	17.192397
32.565421	1205.648529	17.197415
32.405711	1217.325244	17.202432
32.935226	1219.833319	17.207450
32.874415	1219.536747	17.212467
32.748966	1221.992801	17.217485
32.906714	1229.233051	17.222503
33.214043	1235.957542	17.227520
32.832690	1223.144296	17.232538
33.009618	1216.429198	17.237555
32.980276	1224.269980	17.242573
33.067658	1222.810901	17.247591
33.244297	1229.947201	17.252608
33.033436	1222.538592	17.257626
33.174549	1214.449967	17.262643
32.800242	1230.578606	17.267661
33.187347	1218.831590	17.272679
33.063224	1237.903385	17.277696
32.885061	1236.602679	17.282714
33.180611	1223.427747	17.287731
33.253857	1225.404529	17.292749
33.535416	1228.222865	17.297767
33.322504	1236.262833	17.302784
33.220977	1230.266726	17.307802
33.179124	1225.665658	17.312819
32.960898	1227.849059	17.317837
33.367076	1240.898321	17.322855
33.354786	1252.315266	17.327872
33.396440	1256.035918	17.332890
33.538078	1244.756552	17.337907
33.462417	1248.470336	17.342925
33.527220	1252.133710	17.347943
33.463129	1248.978380	17.352960
33.830470	1251.499245	17.357978
34.151620	1244.928804	17.362995
33.396756	1249.105624	17.368013
33.593207	1250.015337	17.373031
33.896692	1251.372202	17.378048
33.780047	1258.911085	17.383066
33.995288	1242.794770	17.388083
33.915198	1252.581255	17.393101
34.156714	1246.856456	17.398119
34.222216	1244.198394	17.403136
33.834434	1249.592696	17.408154
34.150995	1236.572259	17.413171
34.102152	1243.595564	17.418189
34.461626	1260.997871	17.423207
34.339306	1251.413565	17.428224
34.055251	1249.308908	17.433242
33.907041	1247.403882	17.438259
34.252351	1253.099908	17.443277
34.562157	1257.870499	17.448295
34.236265	1265.151823	17.453312
34.050600	1265.796345	17.458330
34.662463	1266.751430	17.463347
34.224248	1266.179460	17.468365
34.505169	1261.499407	17.473383
34.059289	1270.693092	17.478400
34.627947	1263.645191	17.483418
34.878941	1264.656816	17.488435
34.579413	1255.816669	17.493453
34.874259	1257.540975	17.498471
34.922962	1255.084368	17.503488
34.836075	1264.550020	17.508506
34.857455	1259.579260	17.513523
34.961748	1263.905506	17.518541
35.064189	1252.881595	17.523559
34.960137	1261.993315	17.528576
34.529414	1260.353466	17.533594
35.032410	1258.964972	17.538611
35.108379	1259.994552	17.543629
35.037491	1263.792801	17.548647
34.902586	1266.105170	17.553664
34.834162	1267.545553	17.558682
35.325684	1258.278495	17.563699
35.317773	1254.085528	17.568717
34.882699	1266.070516	17.573735
34.755234	1262.492750	17.578752
34.701623	1263.851914	17.583770
35.213018	1284.414777	17.588787
35.284941	1295.035883	17.593805
35.496528	1284.730184	17.598823
35.402808	1285.167789	17.603840
35.397495	1293.121606	17.608858
35.654186	1285.522946	17.613875
35.295091	1288.984488	17.618893
35.785507	1286.641715	17.623911
35.766024	1290.605492	17.628928
35.161973	1290.510803	17.633946
35.638712	1284.263123	17.638963
35.483914	1283.327998	17.643981
35.495055	1276.784025	17.648999
35.776663	1286.147770	17.654016
35.435907	1285.046112	17.659034
35.895530	1277.491403	17.664051
35.843093	1281.640230	17.669069
35.558365	1283.875085	17.674087
35.677872	1284.534913	17.679104
35.625156	1294.806303	17.684122
36.090934	1318.406052	17.689139
35.868820	1316.155976	17.694157
36.024804	1308.301674	17.699175
36.025683	1307.509421	17.704192
36.169406	1314.758214	17.709210
36.150066	1316.724265	17.714227
36.136533	1313.501039	17.719245
36.368308	1301.143963	17.724263
36.208743	1307.600792	17.729280
36.236081	1309.338613	17.734298
36.452421	1306.656909	17.739315
36.296645	1315.170820	17.744333
36.207994	1313.177557	17.749351
36.332628	1304.867401	17.754368
36.136297	1309.925599	17.759386
36.263006	1309.883680	17.764403
36.250826	1312.729116	17.769421
36.123669	1329.516583	17.774439
36.783560	1325.843847	17.779456
36.390427	1335.079795	17.784474
36.855513	1326.880397	17.789491
36.829332	1325.401231	17.794509
36.799975	1321.498800	17.799527
36.811092	1321.639101	17.804544
36.761059	1319.693437	17.809562
36.936189	1324.289479	17.814579
36.702710	1324.001023	17.819597
36.893627	1322.711915	17.824615
36.900607	1321.492653	17.829632
36.904570	1334.444048	17.834650
37.219988	1334.423058	17.839667
36.916279	1338.434534	17.844685
36.786973	1336.182539	17.849703
36.941711	1334.675026	17.854720
36.667852	1341.929293	17.859738
36.863703	1346.613616	17.864755
36.931243	1356.152956	17.869773
37.168030	1363.961570	17.874791
37.516965	1356.638775	17.879808
37.070574	1362.345265	17.884826
37.733409	1354.932262	17.889843
37.648575	1357.934262	17.894861
37.408403	1356.472841	17.899879
37.615946	1346.767371	17.904896
37.539663	1350.437090	17.909914
37.569609	1348.886010	17.914931
37.570730	1357.457413	17.919949
37.536353	1353.959722	17.924967
37.683424	1348.091891	17.929984
37.686684	1353.456515	17.935002
38.164824	1352.554769	17.940019
37.789079	1350.129934	17.945037
38.068955	1355.684760	17.950055
38.466670	1344.362054	17.955072
38.053791	1356.258413	17.960090
37.913967	1350.634356	17.965107
38.131222	1351.906904	17.970125
37.848710	1340.498264	17.975143
38.331857	1344.569504	17.980160
38.052347	1354.128502	17.985178
38.162969	1349.225789	17.990195
37.837231	1342.699858	17.995213
38.044895	1344.955408	18.000231
38.023408	1338.157737	18.005248
37.836198	1343.381780	18.010266
37.898404	1349.459880	18.015283
38.280180	1351.388336	18.020301
37.833579	1351.518297	18.025319
38.131387	1368.308649	18.030336
38.226580	1369.855955	18.035354
38.704743	1373.621855	18.040371
38.444943	1378.443852	18.045389
38.279473	1378.296225	18.050407
38.499749	1373.313206	18.055424
38.556038	1372.386031	18.060442
38.823521	1370.829291	18.065459
38.773716	1371.638731	18.070477
38.808076	1368.325937	18.075495
39.004379	1368.686544	18.080512
38.581590	1369.573358	18.085530
38.741396	1367.351804	18.090547
39.152511	1369.695407	18.095565
38.494149	1364.947888	18.100583
39.124603	1383.769063	18.105600
38.875940	1384.300377	18.110618
38.694647	1388.822884	18.115635
39.035452	1384.490040	18.120653
39.190077	1381.713849	18.125671
39.261277	1378.584638	18.130688
39.057187	1380.099937	18.135706
39.254220	1374.934358	18.140723
39.598061	1381.659496	18.145741
39.455574	1387.996908	18.150759
39.599727	1379.188175	18.155776
39.391182	1381.265932	18.160794
39.338111	1377.045296	18.165811
39.673276	1372.221010	18.170829
39.570425	1378.927767	18.175847
39.536416	1375.120731	18.180864
39.443518	1380.976979	18.185882
39.561492	1375.072670	18.190899
39.963054	1380.254972	18.195917
39.753604	1378.359526	18.200935
39.631593	1369.005493	18.205952
39.803654	1382.527060	18.210970
39.365368	1382.075023	18.215987
39.230433	1378.018699	18.221005
39.478244	1387.974801	18.226023
40.034542	1394.546731	18.231040
40.401789	1400.921054	18.236058
39.912290	1406.337651	18.241075
39.699679	1401.772759	18.246093
39.889009	1409.872865	18.251111
40.195831	1405.002516	18.256128
40.133116	1402.516006	18.261146
40.157311	1402.619543	18.266163
40.427094	1412.310271	18.271181
40.238317	1404.607778	18.276199
40.261835	1394.934271	18.281216
40.311369	1401.307877	18.286234
40.385571	1401.166882	18.291251
40.425270	1399.806783	18.296269
40.164591	1405.099162	18.301287
40.000281	1398.131332	18.306304
40.280883	1417.013669	18.311322
40.466106	1415.772786	18.316339
41.102694	1416.985951	18.321357
40.572823	1428.853349	18.326375
41.083593	1424.149866	18.331392
40.917419	1420.909509	18.336410
40.945664	1417.411462	18.341427
41.101525	1412.807772	18.346445
41.173099	1408.930535	18.351463
41.187910	1394.404529	18.356480
41.330034	1380.666513	18.361498
40.884914	1385.097805	18.366515
40.874919	1382.075993	18.371533
40.721579	1386.351112	18.376551
40.956027	1398.632096	18.381568
41.308915	1410.607338	18.386586
40.970318	1414.586426	18.391603
41.279475	1415.112398	18.396621
41.467775	1413.072575	18.401639
41.578540	1407.885788	18.406656
41.521409	1401.295659	18.411674
41.323429	1407.714359	18.416691
41.374970	1401.940377	18.421709
41.223541	1405.606101	18.426727
41.558594	1404.436423	18.431744
41.450516	1399.971924	18.436762
41.466432	1398.650266	18.441779
41.407062	1399.107739	18.446797
41.149356	1413.435158	18.451815
41.577679	1416.056951	18.456832
41.902845	1417.536671	18.461850
41.565106	1427.505638	18.466867
41.757480	1428.236109	18.471885
41.724482	1425.833307	18.476903
42.180026	1429.463900	18.481920
41.965361	1430.715760	18.486938
41.795857	1433.705791	18.491955
41.915858	1431.244300	18.496973
42.099883	1432.616740	18.501991
41.974341	1432.248252	18.507008
41.861815	1429.400294	18.512026
41.896508	1439.979981	18.517043
42.337696	1436.786479	18.522061
42.038085	1447.358584	18.527079
42.443384	1463.273762	18.532096
42.204979	1462.976607	18.537114
42.067263	1460.624923	18.542131
42.748408	1453.448865	18.547149
42.795241	1467.368832	18.552167
42.578215	1446.150587	18.557184
42.703819	1446.613795	18.562202
42.484689	1458.719720	18.567219
42.406277	1455.724395	18.572237
42.635590	1457.298035	18.577255
42.894888	1453.069468	18.582272
43.054565	1452.397503	18.587290
42.937205	1455.148982	18.592307
43.009895	1447.326605	18.597325
42.686897	1457.785610	18.602343
42.724357	1451.912826	18.607360
42.424705	1452.931838	18.612378
42.434070	1450.367752	18.617395
42.879980	1459.140929	18.622413
42.811708	1481.467502	18.627431
43.102153	1472.964023	18.632448
42.971555	1478.854613	18.637466
43.131722	1486.624791	18.642483
42.874192	1479.829333	18.647501
42.714845	1482.628422	18.652519
43.225535	1493.512279	18.657536
43.521885	1504.458128	18.662554
43.464506	1507.566310	18.667571
43.491493	1502.730310	18.672589
43.861046	1501.937093	18.677607
43.714304	1499.009275	18.682624
43.788558	1503.261387	18.687642
43.818535	1498.652150	18.692659
44.092948	1486.676450	18.697677
44.072820	1500.493320	18.702695
44.121063	1496.821702	18.707712
43.932342	1472.300999	18.712730
43.668114	1469.479959	18.717747
44.164626	1468.259732	18.722765
43.938392	1469.948931	18.727783
44.048532	1486.140759	18.732800
44.298778	1492.097923	18.737818
44.154365	1486.436670	18.742835
44.108124	1481.400699	18.747853
44.219890	1488.130679	18.752871
44.363922	1496.058031	18.757888
44.281154	1487.000761	18.762906
44.218530	1492.678723	18.767923
44.214773	1493.452550	18.772941
44.355911	1497.104015	18.777959
44.430721	1487.400329	18.782976
44.373342	1481.731753	18.787994
44.345334	1485.188798	18.793011
44.064118	1488.937994	18.798029
44.369378	1488.060171	18.803047
44.751721	1502.798648	18.808064
44.758384	1503.498256	18.813082
44.687609	1517.342010	18.818099
44.794428	1517.268492	18.823117
44.577289	1522.819185	18.828135
44.610856	1521.308550	18.833152
44.546312	1520.548630	18.838170
44.524927	1525.961351	18.843187
44.733963	1526.345215	18.848205
44.766903	1525.017724	18.853223
44.745072	1539.245168	18.858240
45.128332	1542.514705	18.863258
44.995115	1546.789865	18.868275
45.284951	1544.219695	18.873293
45.147532	1548.975223	18.878311
45.160513	1545.817233	18.883328
45.517037	1542.185672	18.888346
45.218141	1554.102176	18.893363
45.357041	1543.391128	18.898381
45.195541	1549.851503	18.903399
45.087053	1554.552004	18.908416
45.481512	1558.974879	18.913434
45.576793	1568.491050	18.918451
45.645850	1567.082154	18.923469
45.846203	1566.634199	18.928487
45.680475	1570.630420	18.933504
46.092526	1566.207470	18.938522
46.002183	1565.019220	18.943539
45.754412	1563.748332	18.948557
46.236145	1554.842438	18.953575
46.015131	1566.642600	18.958592
46.131621	1555.149215	18.963610
45.773423	1568.555176	18.968627
45.924308	1562.992807	18.973645
45.994195	1571.058049	18.978663
45.975509	1565.291861	18.983680
46.119698	1563.915378	18.988698
45.881572	1571.400837	18.993715
46.235233	1573.712442	18.998733
46.620979	1582.078515	19.003751
46.133749	1588.706711	19.008768
46.753148	1590.935655	19.013786
46.446549	1594.275414	19.018803
46.615618	1582.963134	19.023821
46.829152	1582.491021	19.028839
46.609204	1583.163016	19.033856
46.553913	1579.311932	19.038874
46.690476	1585.053395	19.043891
46.739998	1575.397807	19.048909
47.417540	1575.891315	19.053927
46.981007	1578.964235	19.058944
46.907511	1578.764324	19.063962
46.918526	1573.971835	19.068979
46.872503	1562.289301	19.073997
47.370247	1572.537726	19.079015
47.329778	1574.797466	19.084032
47.714810	1566.399051	19.089050
47.245623	1579.112312	19.094067
47.377015	1569.933078	19.099085
47.081378	1570.399169	19.104103
47.088887	1567.267280	19.109120
47.544428	1564.936248	19.114138
47.460109	1574.392193	19.119155
47.295758	1559.786821	19.124173
47.619202	1566.871851	19.129191
47.040115	1578.434616	19.134208
47.421444	1574.442536	19.139226
47.435162	1588.866433	19.144243
47.590864	1587.374529	19.149261
47.764666	1589.935234	19.154279
47.611288	1598.344756	19.159296
47.518337	1586.098325	19.164314
47.777761	1593.404847	19.169331
47.854768	1600.077195	19.174349
48.307708	1615.369627	19.179367
48.141911	1621.852793	19.184384
48.365127	1611.440938	19.189402
48.262665	1610.295611	19.194419
48.214556	1608.349614	19.199437
48.507448	1613.381743	19.204455
48.012147	1602.956227	19.209472
48.420900	1607.279040	19.214490
48.444303	1613.038241	19.219507
48.538411	1614.412159	19.224525
48.485887	1611.662076	19.229543
48.208475	1618.068048	19.234560
48.573472	1612.487898	19.239578
48.504789	1620.862069	19.244595
48.631314	1622.701151	19.249613
48.896572	1613.204258	19.254631
48.342537	1621.758620	19.259648
48.677742	1620.311177	19.264666
48.517116	1619.878750	19.269683
48.759091	1613.699299	19.274701
49.012033	1631.831914	19.279719
48.645927	1646.056574	19.284736
49.085269	1643.371442	19.289754
48.875591	1641.270864	19.294771
49.008978	1648.442512	19.299789
48.784117	1643.737457	19.304807
48.744612	1646.849175	19.309824
48.984480	1640.389162	19.314842
49.128385	1660.353588	19.319859
49.036276	1668.046598	19.324877
49.533765	1660.832958	19.329895
49.580248	1671.814901	19.334912
49.742095	1670.028519	19.339930
49.591228	1671.699616	19.344947
49.612903	1671.065044	19.349965
49.919950	1666.204058	19.354983
49.559466	1668.109980	19.360000
49.928913	1668.408751	19.365018
49.563018	1672.786672	19.370035
49.747208	1664.637443	19.375053
49.806253	1669.766190	19.380071
49.856169	1669.815203	19.385088
50.049390	1660.733540	19.390106
50.080485	1665.667837	19.395123
49.410982	1671.564023	19.400141
49.956098	1685.570203	19.405159
49.818908	1691.146295	19.410176
50.387416	1688.986908	19.415194
50.264844	1691.874948	19.420211
49.919024	1686.933196	19.425229
50.211597	1688.111913	19.430247
50.384188	1697.808556	19.435264
50.559839	1704.168823	19.440282
50.406250	1712.568963	19.445299
50.482125	1716.581015	19.450317
50.711460	1715.989651	19.455335
50.737306	1709.796689	19.460352
51.005854	1706.144164	19.465370
50.957121	1698.807791	19.470387
51.072067	1704.540056	19.475405
50.965702	1702.420128	19.480423
50.735796	1706.085585	19.485440
50.560694	1705.911060	19.490458
50.642218	1702.694963	19.495475
50.569751	1713.922802	19.500493
50.955922	1714.392533	19.505511
51.192633	1727.310902	19.510528
51.102220	1728.612747	19.515546
51.196317	1731.937092	19.520563
51.285417	1729.199518	19.525581
51.480044	1734.007219	19.530599
51.231002	1730.981774	19.535616
51.484173	1735.388958	19.540634
51.228897	1734.769372	19.545651
51.592505	1749.107017	19.550669
51.700446	1751.722250	19.555687
51.704979	1763.319934	19.560704
51.785300	1746.665690	19.565722
51.984980	1755.499684	19.570739
51.840956	1757.185496	19.575757
52.112485	1741.792111	19.580775
52.159266	1744.259124	19.585792
52.105364	1750.472323	19.590810
52.334480	1743.041904	19.595827
52.540193	1749.018755	19.600845
52.375302	1732.058938	19.605863
52.423130	1730.505023	19.610880
51.948547	1718.018473	19.615898
52.414627	1726.747594	19.620915
52.650882	1732.659690	19.625933
52.608630	1723.494959	19.630951
52.209047	1726.511618	19.635968
52.719343	1729.884371	19.640986
52.662175	1737.919099	19.646003
52.497930	1736.581459	19.651021
52.393592	1738.967999	19.656039
52.509743	1738.223942	19.661056
52.614950	1748.234148	19.666074
52.836151	1736.938851	19.671091
52.603656	1739.569547	19.676109
52.885566	1737.458214	19.681127
52.898004	1740.312485	19.686144
52.899637	1738.440737	19.691162
52.803109	1745.547454	19.696179
53.234627	1763.241942	19.701197
53.314949	1758.362801	19.706215
53.111235	1769.803755	19.711232
53.275927	1765.757207	19.716250
53.714587	1761.674048	19.721267
53.615720	1765.965970	19.726285
53.805637	1761.571465	19.731303
53.572158	1768.093692	19.736320
53.805253	1766.412910	19.741338
53.973573	1764.745433	19.746355
53.648040	1760.753600	19.751373
53.533812	1763.864422	19.756391
53.613669	1757.988051	19.761408
53.607416	1756.259558	19.766426
54.292397	1752.412382	19.771443
53.943019	1753.073102	19.776461
54.058249	1754.816132	19.781479
54.046033	1765.867295	19.786496
54.061668	1761.686300	19.791514
54.742956	1758.590834	19.796531
54.171488	1760.441453	19.801549
54.292919	1754.277684	19.806567
53.674363	1760.380526	19.811584
53.573333	1760.005034	19.816602
53.988106	1776.720637	19.821619
54.074619	1790.934461	19.826637
54.474214	1788.334436	19.831655
54.492234	1790.944826	19.836672
54.282732	1789.121933	19.841690
54.628111	1781.906828	19.846707
54.654049	1795.442134	19.851725
55.197087	1792.652365	19.856743
55.275265	1806.835948	19.861760
55.002898	1791.357310	19.866778
54.822479	1781.254766	19.871795
54.894725	1796.812140	19.876813
55.250439	1796.333526	19.881831
55.036785	1794.678552	19.886848
55.188267	1798.640905	19.891866
55.208795	1798.375764	19.896883
55.008180	1805.754450	19.901901
55.060973	1809.688083	19.906919
55.072936	1796.150035	19.911936
55.257879	1801.063421	19.916954
55.136850	1813.921129	19.921971
55.159498	1821.832928	19.926989
55.711717	1826.376331	19.932007
55.934697	1827.158833	19.937024
55.862785	1836.631908	19.942042
56.085712	1833.879663	19.947059
55.549053	1836.116183	19.952077
55.857995	1827.698009	19.957095
55.910486	1824.742077	19.962112
55.794614	1827.285081	19.967130
55.802587	1830.717620	19.972147
55.604843	1827.643092	19.977165
55.828761	1832.544068	19.982183
55.935606	1837.356083	19.987200
56.262464	1846.634133	19.992218
56.245858	1841.202070	19.997235
56.223107	1847.845955	20.002253
56.504110	1852.056290	20.007271
56.443285	1857.339581	20.012288
56.644527	1861.347804	20.017306
56.476373	1846.837474	20.022323
56.446960	1856.742590	20.027341
56.529913	1850.458576	20.032359
56.573084	1856.293660	20.037376
56.446442	1854.681856	20.042394
56.924722	1858.731886	20.047411
56.648681	1876.288016	20.052429
57.004292	1869.172266	20.057447
57.265566	1872.590375	20.062464
56.794316	1891.953955	20.067482
57.142431	1872.423512	20.072499
56.686439	1873.691119	20.077517
56.971256	1871.131157	20.082535
57.287424	1871.817004	20.087552
57.048807	1882.613354	20.092570
57.531349	1889.061315	20.097587
57.495814	1907.782246	20.102605
57.691188	1887.770750	20.107623
57.812832	1895.531361	20.112640
57.619674	1904.906695	20.117658
57.469380	1906.063288	20.122675
57.505968	1902.797387	20.127693
57.714352	1902.799480	20.132711
58.125659	1895.633966	20.137728
57.568973	1891.451084	20.142746
57.861887	1888.331232	20.147763
57.948993	1903.075268	20.152781
57.915969	1909.282095	20.157799
58.327630	1907.188286	20.162816
58.286611	1915.681346	20.167834
58.370579	1912.509013	20.172851
58.169761	1915.362007	20.177869
58.620987	1922.569181	20.182887
58.541473	1908.919139	20.187904
58.530990	1917.148619	20.192922
58.202174	1904.503389	20.197939
58.440846	1910.093249	20.202957
58.708847	1895.565042	20.207975
58.456258	1903.895569	20.212992
58.844284	1921.455005	20.218010
59.359557	1926.042095	20.223027
59.019012	1920.152637	20.228045
59.054516	1906.636066	20.233063
59.538587	1909.608989	20.238080
58.847916	1911.314185	20.243098
58.658641	1912.921888	20.248115
58.992124	1932.724362	20.253133
59.170689	1932.844745	20.258151
59.264020	1932.356740	20.263168
59.212325	1926.018050	20.268186
59.548396	1923.945551	20.273203
59.375169	1922.789199	20.278221
58.885083	1928.856188	20.283239
59.547644	1933.486481	20.288256
59.536885	1939.270076	20.293274
59.944963	1949.917805	20.298291
59.558299	1954.687242	20.303309
59.643750	1953.686035	20.308327
59.891602	1952.053421	20.313344
59.643060	1956.570826	20.318362
59.916868	1951.200535	20.323379
60.111238	1956.327098	20.328397
59.878009	1951.414973	20.333415
60.392994	1942.664638	20.338432
60.149443	1948.547830	20.343450
60.113481	1954.205980	20.348467
60.270476	1976.270640	20.353485
60.455910	1974.433192	20.358503
60.260451	1971.702291	20.363520
60.454918	1972.138944	20.368538
60.668447	1969.779501	20.373555
60.757772	1969.812873	20.378573
60.571526	1974.778151	20.383591
60.973835	1972.559558	20.388608
60.941336	1967.436083	20.393626
61.111482	1961.059468	20.398643
60.698671	1968.657675	20.403661
61.038839	1969.103061	20.408679
60.757108	1958.205184	20.413696
60.987538	1977.499948	20.418714
61.093432	1980.794087	20.423731
61.433421	1990.590905	20.428749
61.103413	1993.596706	20.433767
61.170110	1987.924310	20.438784
61.634737	1997.035675	20.443802
61.053855	1990.480047	20.448819
61.236161	1992.543978	20.453837
61.678263	2007.093613	20.458855
61.510686	2014.331498	20.463872
61.283765	2018.425775	20.468890
61.578954	2015.690585	20.473907
61.845747	2013.865634	20.478925
61.747794	2021.458717	20.483943
62.362011	2017.452146	20.488960
62.071389	2017.478768	20.493978
62.051130	2012.927767	20.498995
62.127817	2021.749602	20.504013
62.482283	2036.855835	20.509031
62.347455	2033.193854	20.514048
62.429282	2034.733844	20.519066
62.823490	2025.386959	20.524083
62.920593	2032.561290	20.529101
62.483754	2033.178913	20.534119
62.576088	2020.555988	20.539136
62.914297	2029.422066	20.544154
63.006483	2032.727831	20.549171
63.096267	2030.128970	20.554189
62.617901	2039.716331	20.559207
62.741423	2027.025394	20.564224
63.187743	2039.570293	20.569242
62.788670	2026.749776	20.574259
63.099351	2021.297941	20.579277
63.004720	2027.814289	20.584295
62.935457	2026.843629	20.589312
63.087304	2028.805029	20.594330
62.941760	2037.582789	20.599347
62.870942	2047.431376	20.604365
63.090235	2058.815708	20.609383
63.181282	2054.335627	20.614400
63.431497	2060.403449	20.619418
63.466727	2068.206078	20.624435
63.768731	2078.400248	20.629453
63.616504	2086.408996	20.634471
63.600626	2079.518639	20.639488
63.632733	2082.862230	20.644506
63.822522	2086.023314	20.649523
63.857705	2082.786005	20.654541
64.045576	2086.357678	20.659559
64.455454	2080.792446	20.664576
63.920922	2081.939816	20.669594
63.765641	2086.423706	20.674611
64.070958	2088.705080	20.679629
64.118171	2101.662878	20.684647
64.324920	2108.375053	20.689664
64.521394	2107.160766	20.694682
64.476886	2117.491306	20.699699
64.605850	2107.194926	20.704717
64.756157	2111.381613	20.709735
64.946825	2110.218733	20.714752
65.123198	2112.807516	20.719770
65.101681	2112.911907	20.724787
65.298217	2103.438148	20.729805
64.920642	2103.926557	20.734823
65.404134	2114.508915	20.739840
65.598637	2126.446332	20.744858
65.124331	2105.630564	20.749875
65.634916	2107.851376	20.754893
65.403969	2114.206059	20.759911
65.729202	2120.558819	20.764928
65.648261	2118.318083	20.769946
65.859182	2112.837665	20.774963
65.920679	2097.012939	20.779981
65.534519	2100.321071	20.784999
65.661716	2104.909044	20.790016
65.805528	2114.165415	20.795034
65.696728	2117.969785	20.800051
65.821597	2121.216792	20.805069
65.942693	2127.942394	20.810087
66.054807	2119.229845	20.815104
65.734712	2118.453128	20.820122
65.918109	2114.059558	20.825139
66.159179	2127.933827	20.830157
66.011586	2134.594222	20.835175
66.218086	2128.963000	20.840192
66.534728	2132.583942	20.845210
66.418835	2130.017291	20.850227
66.506159	2135.555188	20.855245
66.458112	2140.328431	20.860263
66.716681	2155.392979	20.865280
66.704336	2162.635008	20.870298
66.749975	2161.611622	20.875315
66.902851	2155.524848	20.880333
66.857063	2158.350435	20.885351
67.051060	2160.595606	20.890368
66.965147	2158.021098	20.895386
66.900493	2164.747412	20.900403
67.284041	2167.530983	20.905421
67.007290	2187.978507	20.910439
67.304141	2185.148349	20.915456
67.266528	2187.896913	20.920474
67.160485	2184.899483	20.925491
67.415884	2184.035753	20.930509
67.631941	2193.981499	20.935527
67.582505	2194.895069	20.940544
67.694025	2204.929790	20.945562
67.667268	2203.523232	20.950579
68.282475	2203.998123	20.955597
68.818152	2206.584281	20.960615
68.247837	2198.979095	20.965632
68.585991	2208.403900	20.970650
68.417208	2194.060661	20.975667
68.666477	2183.833759	20.980685
68.342019	2182.779986	20.985703
68.605949	2180.917594	20.990720
68.552985	2175.825672	20.995738
68.209420	2178.940935	21.000755
68.581828	2189.875288	21.005773
68.481880	2199.097304	21.010791
68.931720	2205.484225	21.015808
68.586354	2199.996254	21.020826
68.535086	2202.431350	21.025843
68.735404	2199.960328	21.030861
68.306956	2200.043260	21.035879
69.180197	2204.990944	21.040896
68.840334	2222.327015	21.045914
68.759294	2236.128745	21.050931
69.388511	2230.431263	21.055949
69.247734	2236.301602	21.060967
69.124400	2237.693856	21.065984
69.285508	2233.562550	21.071002
69.105823	2242.948573	21.076019
69.386790	2246.625626	21.081037
69.414181	2260.688124	21.086055
69.777495	2247.419768	21.091072
69.834742	2252.517402	21.096090
70.001879	2255.385391	21.101107
69.888568	2250.006228	21.106125
69.420867	2251.717549	21.111143
70.137155	2262.026814	21.116160
70.386359	2265.639412	21.121178
70.389453	2266.626815	21.126195
70.528355	2271.364490	21.131213
70.397610	2270.659094	21.136231
70.744921	2279.337661	21.141248
70.870242	2267.340616	21.146266
70.880533	2267.638860	21.151283
71.114779	2263.054233	21.156301
70.820887	2266.597271	21.161319
70.922107	2269.614458	21.166336
71.052464	2257.824934	21.171354
71.163652	2265.101304	21.176371
71.205097	2266.044824	21.181389
71.228299	2263.860344	21.186407
71.060818	2258.685344	21.191424
71.509809	2262.500192	21.196442
71.088646	2264.273657	21.201459
71.215840	2267.804376	21.206477
70.936950	2264.897135	21.211495
71.168090	2268.023368	21.216512
71.668733	2276.027751	21.221530
71.550398	2285.404185	21.226547
71.494286	2279.110248	21.231565
71.667497	2282.040411	21.236583
71.870001	2287.623432	21.241600
71.725828	2286.793895	21.246618
71.666506	2280.068073	21.251635
71.788503	2276.220623	21.256653
72.000850	2299.804565	21.261671
71.802973	2303.600837	21.266688
72.203756	2306.621595	21.271706
72.123029	2311.444189	21.276723
71.939852	2308.752341	21.281741
72.189069	2322.833787	21.286759
72.588098	2339.214678	21.291776
73.079306	2332.478330	21.296794
72.724165	2341.598375	21.301811
73.194397	2342.553623	21.306829
72.934347	2344.144048	21.311847
72.883012	2338.146017	21.316864
73.286633	2342.775958	21.321882
73.311355	2338.836427	21.326899
73.282523	2338.152935	21.331917
72.932085	2343.005169	21.336935
72.923285	2344.227992	21.341952
72.934778	2329.487133	21.346970
73.192581	2339.249677	21.351987
73.361667	2338.440493	21.357005
73.599721	2353.653604	21.362023
74.028340	2347.690839	21.367040
74.156147	2335.652330	21.372058
74.231845	2352.670929	21.377075
74.192303	2331.010375	21.382093
73.961051	2326.605972	21.387111
73.869484	2325.269525	21.392128
74.028525	2330.420668	21.397146
74.339366	2337.533229	21.402163
74.229543	2340.160573	21.407181
74.334600	2343.858894	21.412199
74.228816	2340.763557	21.417216
74.837612	2336.757766	21.422234
74.111360	2348.489260	21.427251
74.395083	2344.528085	21.432269
74.514622	2346.027477	21.437287
74.245912	2347.161620	21.442304
74.709731	2357.523121	21.447322
74.668823	2360.221730	21.452339
74.763061	2356.435422	21.457357
74.765820	2357.665904	21.462375
74.535311	2362.480416	21.467392
74.961946	2381.473449	21.472410
75.259509	2390.093585	21.477427
75.087144	2384.827786	21.482445
75.012992	2390.416310	21.487463
75.190031	2403.896839	21.492480
75.477407	2400.986072	21.497498
75.140319	2415.746491	21.502515
75.363692	2408.079988	21.507533
75.619086	2414.529011	21.512551
75.558752	2421.816536	21.517568
75.766385	2431.069384	21.522586
76.001240	2436.199211	21.527603
76.221035	2438.471937	21.532621
76.161697	2439.914146	21.537639
76.247752	2447.784725	21.542656
75.889559	2444.154498	21.547674
75.721392	2445.266583	21.552691
75.791002	2455.835085	21.557709
76.412919	2460.500291	21.562727
76.261673	2465.030984	21.567744
76.502257	2461.916077	21.572762
76.579502	2475.200834	21.577779
76.935511	2472.929468	21.582797
77.117832	2480.131657	21.587815
76.952324	2494.767418	21.592832
77.373993	2486.659515	21.597850
77.480355	2489.249854	21.602867
77.614393	2484.453629	21.607885
77.531875	2483.216748	21.612903
77.401644	2499.248314	21.617920
77.380726	2487.233006	21.622938
77.384919	2489.662607	21.627955
77.854409	2489.983595	21.632973
77.709660	2485.799154	21.637991
77.959511	2493.704058	21.643008
78.043660	2487.829933	21.648026
77.640028	2486.419276	21.653043
77.885454	2487.756930	21.658061
77.765698	2482.621730	21.663079
77.754149	2495.765762	21.668096
77.860804	2503.551078	21.673114
77.976788	2512.594241	21.678131
78.028498	2512.283174	21.683149
78.346342	2503.689702	21.688167
78.107491	2517.257568	21.693184
77.944740	2519.097880	21.698202
78.346836	2528.298218	21.703219
78.294698	2542.105123	21.708237
78.657144	2543.667471	21.713255
78.434125	2548.054778	21.718272
79.105444	2548.154776	21.723290
78.982451	2553.561633	21.728307
79.117237	2560.761833	21.733325
79.351481	2558.771496	21.738343
78.937784	2557.356098	21.743360
79.362236	2557.823014	21.748378
79.193789	2560.775190	21.753395
79.354093	2568.545817	21.758413
79.412688	2571.809601	21.763431
79.456898	2580.504240	21.768448
79.718394	2589.963350	21.773466
80.005109	2582.391003	21.778483
79.803480	2585.537752	21.783501
80.092362	2586.265778	21.788519
79.920482	2587.088086	21.793536
80.091666	2598.155212	21.798554
80.473360	2611.550179	21.803571
80.688806	2599.620854	21.808589
81.165554	2599.359972	21.813607
80.812270	2586.964274	21.818624
80.454747	2583.690561	21.823642
80.763253	2590.996115	21.828659
80.978812	2602.182539	21.833677
81.743993	2586.313414	21.838695
81.483108	2576.273527	21.843712
81.149773	2563.379202	21.848730
80.983261	2566.955996	21.853747
81.337478	2565.499190	21.858765
81.527669	2558.683674	21.863783
81.243031	2556.964001	21.868800
81.574373	2568.709841	21.873818
81.618100	2575.371986	21.878835
81.664575	2587.673767	21.883853
81.820541	2591.490410	21.888871
81.664176	2590.618582	21.893888
81.857566	2589.824517	21.898906
81.874623	2580.233443	21.903923
81.659087	2591.061319	21.908941
81.842670	2582.899146	21.913959
81.667531	2586.597229	21.918976
81.670242	2598.202050	21.923994
81.763744	2611.099308	21.929011
82.117975	2618.397709	21.934029
82.165758	2613.094196	21.939047
81.928885	2628.050550	21.944064
82.163554	2638.492302	21.949082
82.257776	2642.239724	21.954099
82.086812	2641.013534	21.959117
82.543746	2659.402441	21.964135
82.706369	2663.827198	21.969152
82.558921	2673.385140	21.974170
83.131976	2677.527821	21.979187
83.076027	2677.539768	21.984205
83.100463	2669.036373	21.989223
82.848345	2686.213958	21.994240
82.886039	2686.526852	21.999258
83.346416	2689.039662	22.004275
82.977074	2697.616091	22.009293
83.197852	2701.580412	22.014311
83.466972	2723.855668	22.019328
83.988468	2712.487463	22.024346
84.503512	2707.388459	22.029363
84.048620	2717.032467	22.034381
84.548245	2710.865931	22.039399
84.186896	2715.442229	22.044416
84.851624	2718.055587	22.049434
84.543693	2707.877812	22.054451
84.458273	2711.583958	22.059469
84.522504	2702.720820	22.064487
84.532266	2706.648766	22.069504
84.741411	2707.329322	22.074522
84.850620	2710.443174	22.079539
84.839806	2714.835149	22.084557
84.996785	2706.995863	22.089575
84.713732	2700.809926	22.094592
84.964365	2696.677113	22.099610
85.214121	2706.289621	22.104627
85.154719	2714.707033	22.109645
85.455909	2709.679408	22.114663
85.358394	2725.153717	22.119680
85.041102	2730.054515	22.124698
85.387725	2728.169645	22.129715
85.528034	2728.829424	22.134733
85.379381	2721.306293	22.139751
85.070701	2736.608542	22.144768
85.279365	2748.316909	22.149786
85.955984	2747.926869	22.154803
85.982365	2746.884374	22.159821
85.867594	2753.612447	22.164839
85.748273	2775.651943	22.169856
85.729883	2767.142587	22.174874
86.198256	2769.095509	22.179891
86.129221	2788.425439	22.184909
86.666542	2794.890396	22.189927
86.668827	2798.567038	22.194944
86.705285	2796.642381	22.199962
86.894964	2788.933653	22.204979
86.810480	2794.618607	22.209997
87.348605	2799.480090	22.215015
87.490862	2799.672450	22.220032
87.060714	2788.939348	22.225050
87.803423	2786.796732	22.230067
87.463597	2786.648002	22.235085
87.765266	2790.091521	22.240103
87.738429	2794.621742	22.245120
88.012521	2803.539281	22.250138
87.790394	2792.631558	22.255155
87.808288	2798.710779	22.260173
88.160731	2804.040067	22.265191
88.270418	2807.273796	22.270208
88.190900	2803.240028	22.275226
88.338681	2800.739281	22.280243
88.412572	2801.254816	22.285261
88.373067	2797.713460	22.290279
88.556604	2803.362737	22.295296
88.517791	2794.370513	22.300314
88.630016	2796.382393	22.305331
88.368773	2802.458005	22.310349
88.646542	2800.381918	22.315367
88.585141	2811.936953	22.320384
88.422639	2820.114914	22.325402
88.773470	2831.027791	22.330419
88.506748	2829.002289	22.335437
88.872363	2828.332728	22.340455
89.184989	2840.062741	22.345472
89.058524	2850.687444	22.350490
89.415622	2850.779864	22.355507
89.314972	2866.311597	22.360525
89.325387	2852.015506	22.365543
89.167279	2856.114971	22.370560
88.957546	2870.739027	22.375578
89.788998	2869.295803	22.380595
89.833407	2874.597623	22.385613
90.135550	2876.459821	22.390631
90.275929	2879.556194	22.395648
90.332855	2890.234250	22.400666
90.388739	2891.431195	22.405683
90.441315	2896.674930	22.410701
90.671073	2894.047704	22.415719
90.671559	2895.325921	22.420736
90.993841	2896.957719	22.425754
90.988279	2886.991280	22.430771
90.961196	2886.872456	22.435789
91.122837	2883.851907	22.440807
90.653711	2890.026398	22.445824
90.938740	2889.498867	22.450842
91.458184	2886.343354	22.455859
91.157431	2903.118456	22.460877
91.235122	2907.600767	22.465895
91.475646	2916.207999	22.470912
91.218751	2915.291938	22.475930
91.723962	2911.482157	22.480947
92.004926	2905.166753	22.485965
91.610170	2899.222339	22.490983
91.518150	2925.543887	22.496000
92.168405	2930.599306	22.501018
92.335565	2930.891921	22.506035
91.719518	2933.232539	22.511053
92.261146	2931.115098	22.516071
92.463910	2936.436314	22.521088
92.383003	2951.453718	22.526106
92.668614	2948.053926	22.531123
92.566778	2961.670096	22.536141
92.653766	2956.552870	22.541159
92.734703	2957.543895	22.546176
92.445815	2961.506062	22.551194
93.094279	2974.433414	22.556211
93.255343	2981.778009	22.561229
93.139645	2986.498949	22.566247
93.430236	2987.059444	22.571264
93.301745	2979.675076	22.576282
93.348411	2971.256431	22.581299
93.749554	2981.785925	22.586317
93.788251	2991.232810	22.591335
94.231280	2994.013506	22.596352
94.263292	3008.694487	22.601370
94.381454	3009.117873	22.606387
94.303144	3008.659887	22.611405
94.288104	2998.802184	22.616423
94.420159	2996.281781	22.621440
94.590011	3002.330951	22.626458
94.266192	2993.058187	22.631475
94.432628	3001.869598	22.636493
94.609100	2998.316459	22.641511
94.482441	3002.470998	22.646528
94.275700	3006.817991	22.651546
94.792950	3015.350353	22.656563
94.681574	3022.346275	22.661581
94.907265	3026.148930	22.666599
95.187457	3029.097174	22.671616
94.901993	3033.270288	22.676634
95.382513	3046.738472	22.681651
95.491301	3054.346942	22.686669
95.366381	3050.310763	22.691687
95.601077	3054.307701	22.696704
95.594027	3056.524516	22.701722
96.091478	3045.983650	22.706739
95.768207	3050.816034	22.711757
95.648271	3050.516069	22.716775
96.369942	3066.531452	22.721792
95.729622	3076.703388	22.726810
96.570000	3070.101439	22.731827
96.039276	3076.304581	22.736845
96.068744	3086.223243	22.741863
96.583534	3081.910082	22.746880
96.594595	3086.453377	22.751898
96.656198	3088.637346	22.756915
96.773152	3096.405524	22.761933
96.852725	3085.563980	22.766951
97.096566	3089.906680	22.771968
97.069585	3108.643301	22.776986
97.399281	3115.598561	22.782003
97.280177	3118.129627	22.787021
97.511853	3121.319051	22.792039
97.324088	3117.261140	22.797056
97.588632	3125.384958	22.802074
98.343761	3111.761052	22.807091
98.071384	3104.743207	22.812109
98.285450	3104.605538	22.817127
98.332402	3096.474008	22.822144
98.345049	3099.129618	22.827162
98.380388	3102.873737	22.832179
98.418671	3107.153959	22.837197
98.308860	3114.228577	22.842215
98.616676	3116.121475	22.847232
98.765318	3122.192946	22.852250
98.895371	3120.256747	22.857267
98.921923	3130.867110	22.862285
98.754756	3129.725510	22.867303
98.840542	3131.088224	22.872320
98.845336	3147.736776	22.877338
99.183393	3148.469747	22.882355
99.151868	3154.878770	22.887373
99.044561	3157.799370	22.892391
99.274090	3163.788744	22.897408
99.367059	3176.055237	22.902426
99.659829	3185.557105	22.907443
99.653320	3185.406649	22.912461
99.756234	3174.570864	22.917479
100.077168	3189.209882	22.922496
100.172909	3197.218147	22.927514
100.041635	3204.384539	22.932531
100.020386	3205.659871	22.937549
99.692249	3206.932783	22.942567
99.782425	3212.151782	22.947584
100.605042	3227.829553	22.952602
100.724154	3224.004448	22.957619
100.392408	3241.059314	22.962637
100.540863	3261.428810	22.967655
101.030315	3255.775003	22.972672
100.924577	3269.906490	22.977690
101.105204	3262.981737	22.982707
100.921743	3271.081122	22.987725
100.920428	3276.819479	22.992743
100.884558	3291.489230	22.997760
101.068598	3300.225435	23.002778
101.261311	3314.531138	23.007795
101.754301	3319.794373	23.012813
101.765218	3310.276469	23.017831
102.257908	3304.792579	23.022848
102.030810	3309.145989	23.027866
102.391370	3303.862708	23.032883
102.516461	3310.998446	23.037901
102.476499	3316.932248	23.042919
102.616218	3334.001713	23.047936
102.379871	3336.936246	23.052954
102.588860	3330.900256	23.057971
102.853788	3333.131307	23.062989
102.673949	3334.412557	23.068007
103.071624	3327.715747	23.073024
103.159230	3333.793696	23.078042
103.174113	3350.825921	23.083059
103.330733	3358.723719	23.088077
103.574564	3350.895798	23.093095
103.766776	3353.359185	23.098112
103.553379	3363.287642	23.103130
103.615558	3361.112704	23.108147
103.507852	3359.472546	23.113165
103.582355	3378.695398	23.118183
104.026827	3383.132989	23.123200
104.141598	3387.139321	23.128218
104.201015	3386.845970	23.133235
104.334695	3386.657767	23.138253
104.604095	3388.730310	23.143271
105.082648	3390.975244	23.148288
105.257184	3402.023403	23.153306
105.023819	3383.567197	23.158323
105.146180	3376.891408	23.163341
105.608451	3388.999185	23.168359
105.221693	3376.213649	23.173376
105.623713	3384.180325	23.178394
105.597403	3396.434091	23.183411
105.530725	3386.622142	23.188429
105.478501	3395.234436	23.193447
105.696366	3382.376263	23.198464
105.578927	3398.485530	23.203482
105.775887	3390.601809	23.208499
105.742972	3388.435454	23.213517
106.214086	3398.711196	23.218535
106.187258	3413.284940	23.223552
106.249091	3416.513651	23.228570
106.095462	3422.765145	23.233587
106.509792	3417.467095	23.238605
106.279479	3423.313971	23.243623
106.069114	3416.251569	23.248640
106.276077	3434.620463	23.253658
106.453489	3436.063535	23.258675
106.744224	3448.586453	23.263693
106.579112	3466.666477	23.268711
107.038508	3461.402387	23.273728
107.292493	3465.614180	23.278746
107.478978	3475.041320	23.283763
108.073582	3469.430943	23.288781
107.740071	3489.563730	23.293799
107.915827	3484.255694	23.298816
108.116179	3488.438019	23.303834
108.178325	3483.974738	23.308851
108.419632	3479.707488	23.313869
108.209571	3496.017576	23.318887
108.189362	3483.004095	23.323904
108.129211	3488.622327	23.328922
108.016595	3485.875058	23.333939
108.468589	3503.132484	23.338957
108.382701	3517.605094	23.343975
108.564499	3510.493840	23.348992
108.701018	3511.700288	23.354010
108.657370	3530.572522	23.359027
108.976008	3532.911968	23.364045
108.773118	3541.948791	23.369063
108.998987	3542.001807	23.374080
109.213916	3551.298277	23.379098
109.191507	3566.029269	23.384115
109.547790	3568.040875	23.389133
109.356195	3565.621601	23.394151
109.638007	3565.586944	23.399168
109.802476	3590.565709	23.404186
109.754331	3600.654629	23.409203
110.193072	3595.595742	23.414221
109.535265	3602.314517	23.419239
109.769014	3613.167303	23.424256
110.284257	3619.800150	23.429274
110.324218	3623.300614	23.434291
110.439978	3640.756040	23.439309
110.708801	3649.782141	23.444327
110.474493	3650.974099	23.449344
110.913303	3652.205793	23.454362
110.755138	3672.661666	23.459379
111.481987	3673.292716	23.464397
111.228588	3678.398390	23.469415
111.134567	3672.725395	23.474432
111.374295	3690.041505	23.479450
111.539082	3695.968604	23.484467
111.801858	3693.320309	23.489485
112.129018	3698.117244	23.494503
112.020708	3695.962664	23.499520
112.099619	3703.162606	23.504538
112.065574	3723.602247	23.509555
112.862530	3723.029211	23.514573
112.589693	3721.601116	23.519591
112.444072	3725.105424	23.524608
112.584498	3724.714155	23.529626
112.810313	3738.162790	23.534643
113.248786	3751.644402	23.539661
113.075105	3759.436304	23.544679
113.294910	3751.709823	23.549696
113.474097	3745.975063	23.554714
113.295878	3745.709468	23.559731
113.715056	3750.450968	23.564749
113.622870	3749.029289	23.569767
113.774169	3766.731779	23.574784
113.565801	3768.721398	23.579802
113.744568	3777.319780	23.584819
114.065337	3773.488217	23.589837
114.120648	3789.981095	23.594855
114.001496	3799.229029	23.599872
114.123481	3804.667318	23.604890
114.357892	3804.996759	23.609907
114.623725	3805.450687	23.614925
114.794556	3822.427361	23.619943
114.687014	3825.158721	23.624960
115.052627	3822.238630	23.629978
114.902323	3828.679125	23.634995
115.235477	3829.422364	23.640013
115.570718	3840.559243	23.645031
115.433307	3832.563584	23.650048
115.494981	3840.400714	23.655066
115.502683	3836.457211	23.660083
115.742752	3839.610728	23.665101
115.403237	3859.943717	23.670119
115.882049	3858.511481	23.675136
116.194025	3861.136089	23.680154
116.273005	3865.845696	23.685171
116.529171	3873.646057	23.690189
116.355852	3895.057785	23.695207
116.161054	3894.747438	23.700224
116.776161	3891.235879	23.705242
116.765386	3895.975338	23.710259
117.077788	3888.111192	23.715277
116.767698	3891.568702	23.720295
116.771223	3905.831917	23.725312
117.272530	3918.315858	23.730330
117.035512	3918.485586	23.735347
117.189799	3910.513634	23.740365
117.327709	3932.296446	23.745383
117.482651	3940.362049	23.750400
117.789128	3939.423954	23.755418
117.503265	3942.830332	23.760435
117.637677	3969.682918	23.765453
117.926147	3967.920665	23.770471
117.978798	3976.671468	23.775488
118.291558	3991.441831	23.780506
118.271415	4001.210945	23.785523
118.657064	3996.355964	23.790541
118.400777	4003.147704	23.795559
118.621154	4011.209401	23.800576
118.806236	4027.533812	23.805594
118.606855	4027.817588	23.810611
118.817098	4040.725984	23.815629
119.006407	4049.455413	23.820647
119.297764	4051.562470	23.825664
119.493217	4055.499494	23.830682
119.413790	4067.749410	23.835699
119.574912	4068.813159	23.840717
120.318541	4077.291623	23.845735
120.596474	4077.762602	23.850752
120.912336	4065.349431	23.855770
120.626864	4061.966307	23.860787
120.716451	4060.244673	23.865805
120.787434	4078.383010	23.870823
121.100912	4086.370182	23.875840
121.295095	4078.931655	23.880858
121.538449	4088.807887	23.885875
121.348854	4080.864484	23.890893
121.475602	4083.426608	23.895911
122.014941	4081.340963	23.900928
122.159093	4075.011868	23.905946
121.930987	4075.552658	23.910963
122.268079	4076.797162	23.915981
122.146250	4074.682531	23.920999
122.170577	4083.538830	23.926016
122.250007	4074.716830	23.931034
122.024644	4076.409285	23.936051
122.194888	4068.014959	23.941069
122.399094	4073.516202	23.946087
122.359995	4089.067747	23.951104
122.663178	4085.737590	23.956122
122.615851	4102.111106	23.961139
123.067415	4098.666164	23.966157
123.155909	4099.132102	23.971175
122.956780	4110.040380	23.976192
123.044511	4120.386067	23.981210
123.139712	4128.641031	23.986227
123.204900	4118.104141	23.991245
123.009744	4143.342021	23.996263
123.260671	4150.714047	24.001280
123.469247	4158.613524	24.006298
123.808730	4174.358345	24.011315
123.971598	4173.865701	24.016333
124.385588	4177.891616	24.021351
123.910773	4192.712932	24.026368
124.267307	4199.203567	24.031386
124.220558	4209.706101	24.036403
124.617196	4202.387315	24.041421
124.816417	4212.721901	24.046439
124.727885	4221.760084	24.051456
125.006865	4230.646000	24.056474
124.879211	4235.466987	24.061491
124.924799	4237.142259	24.066509
125.191295	4246.794001	24.071527
125.231350	4257.822717	24.076544
125.636830	4245.890947	24.081562
125.221232	4259.430989	24.086579
125.688494	4275.149566	24.091597
125.681502	4279.389811	24.096615
125.955457	4286.335320	24.101632
126.300095	4305.703065	24.106650
126.109909	4306.856587	24.111667
126.597655	4304.958919	24.116685
126.713931	4313.264325	24.121703
126.837990	4325.280521	24.126720
127.016033	4328.071378	24.131738
127.111980	4339.122952	24.136755
127.099641	4339.279578	24.141773
127.454052	4334.820803	24.146791
127.549206	4360.310210	24.151808
127.742254	4363.291267	24.156826
127.733603	4359.283926	24.161843
127.965670	4360.907899	24.166861
128.096822	4357.027010	24.171879
127.417984	4369.058546	24.176896
128.261867	4378.641996	24.181914
128.276201	4380.069659	24.186931
128.290547	4387.257893	24.191949
128.351976	4399.662728	24.196967
128.687085	4415.392662	24.201984
129.148742	4412.138626	24.207002
129.016755	4408.911309	24.212019
128.853584	4413.220244	24.217037
129.435831	4429.672185	24.222055
129.357092	4441.395111	24.227072
129.436716	4429.192311	24.232090
129.630335	4429.749109	24.237107
129.732182	4445.711315	24.242125
129.992232	4461.629812	24.247143
129.981239	4468.089741	24.252160
130.342224	4460.132514	24.257178
130.478957	4456.657917	24.262195
130.527238	4452.736331	24.267213
131.210912	4459.974400	24.272231
131.526771	4473.516795	24.277248
131.551676	4458.516426	24.282266
131.704535	4456.421845	24.287283
131.487010	4441.345837	24.292301
131.771383	4432.826143	24.297319
131.660775	4433.746252	24.302336
131.507136	4436.121930	24.307354
131.662267	4452.186272	24.312371
131.853292	4456.436570	24.317389
132.049025	4457.485450	24.322407
131.957665	4462.105109	24.327424
132.257836	4461.616199	24.332442
132.186960	4476.674328	24.337459
131.838270	4487.028624	24.342477
132.414504	4494.962186	24.347495
132.287827	4502.743885	24.352512
132.302444	4517.100537	24.357530
132.818420	4522.818219	24.362547
132.896480	4525.741562	24.367565
132.957392	4531.473723	24.372583
132.877073	4552.994758	24.377600
133.333732	4554.400485	24.382618
133.259290	4559.882401	24.387635
133.733265	4575.066737	24.392653
133.751918	4576.427453	24.397671
133.553876	4585.138913	24.402688
133.938038	4584.605276	24.407706
133.923040	4600.787941	24.412723
133.835977	4617.587963	24.417741
133.981793	4611.375212	24.422759
133.819434	4621.763523	24.427776
134.182553	4625.402943	24.432794
133.922451	4641.068497	24.437811
133.888500	4658.958705	24.442829
134.651425	4670.508883	24.447847
134.702099	4679.582301	24.452864
134.878505	4699.153588	24.457882
134.895985	4711.641278	24.462899
135.154735	4726.745824	24.467917
136.030465	4722.827121	24.472935
136.152405	4730.311131	24.477952
136.258332	4729.767420	24.482970
136.797868	4728.442399	24.487987
136.174704	4730.809603	24.493005
137.133571	4735.839286	24.498023
136.838648	4760.522317	24.503040
137.004937	4747.639696	24.508058
137.532548	4752.389727	24.513075
137.402384	4743.363498	24.518093
137.439801	4737.183471	24.523111
137.457989	4751.896437	24.528128
137.319323	4737.596964	24.533146
137.791998	4756.045517	24.538163
137.988707	4773.574578	24.543181
138.024577	4767.060188	24.548199
138.047614	4778.072947	24.553216
138.167393	4774.888191	24.558234
138.121486	4771.278008	24.563251
138.291247	4793.009514	24.568269
138.206310	4798.486833	24.573287
138.401540	4802.051583	24.578304
139.284856	4815.120233	24.583322
139.497321	4829.414570	24.588339
139.372373	4832.230878	24.593357
139.390016	4819.545104	24.598375
139.117921	4826.197581	24.603392
139.504024	4833.368785	24.608410
139.836063	4841.997321	24.613427
139.961391	4844.853335	24.618445
140.234209	4844.902160	24.623463
139.800022	4847.362878	24.628480
140.113953	4848.724703	24.633498
140.198443	4871.994280	24.638515
140.273901	4872.844225	24.643533
140.568605	4865.752635	24.648551
140.694259	4886.591543	24.653568
140.815869	4892.386909	24.658586
140.971296	4890.525463	24.663603
140.905354	4903.206278	24.668621
141.452545	4912.088388	24.673639
141.297757	4921.244620	24.678656
141.578029	4925.881932	24.683674
142.018415	4927.530139	24.688691
141.787786	4947.850438	24.693709
141.931442	4946.398029	24.698727
142.119813	4952.978413	24.703744
142.367014	4956.071034	24.708762
142.928832	4963.981810	24.713779
142.783940	4976.264689	24.718797
142.871728	4978.160692	24.723815
143.054057	4981.190879	24.728832
142.981569	4979.545056	24.733850
143.114522	4972.295683	24.738867
142.946418	4987.947121	24.743885
143.416105	4986.693001	24.748903
143.289887	4996.757047	24.753920
143.239158	5004.072513	24.758938
143.572684	5002.243129	24.763955
143.908685	5017.099071	24.768973
144.223445	5014.890679	24.773991
144.328180	5025.521467	24.779008
144.237576	5037.186660	24.784026
144.414097	5041.553006	24.789043
144.446258	5051.241888	24.794061
145.068801	5054.029509	24.799079
144.911136	5067.435041	24.804096
145.079648	5060.615673	24.809114
145.194448	5074.253148	24.814131
145.047677	5076.365835	24.819149
145.548238	5094.990290	24.824167
145.810474	5093.512979	24.829184
146.037753	5086.977958	24.834202
146.367473	5103.050245	24.839219
146.357275	5109.204087	24.844237
146.709177	5096.339490	24.849255
147.043360	5096.849036	24.854272
147.107371	5107.959742	24.859290
147.173427	5098.056627	24.864307
147.248407	5104.152931	24.869325
147.445600	5093.528508	24.874343
147.843888	5097.358225	24.879360
147.630854	5106.892997	24.884378
147.775385	5107.340714	24.889395
147.683036	5125.063759	24.894413
147.720713	5129.076241	24.899431
148.338805	5125.794417	24.904448
148.093231	5130.788788	24.909466
148.560629	5133.711209	24.914483
148.239926	5151.867788	24.919501
148.489959	5157.239073	24.924519
148.558718	5156.925292	24.929536
148.528135	5165.291975	24.934554
148.859804	5172.976899	24.939571
148.980115	5197.232457	24.944589
148.916949	5196.216477	24.949607
149.527372	5197.355109	24.954624
149.118323	5213.331739	24.959642
149.120748	5224.871996	24.964659
149.277084	5243.269592	24.969677
149.856320	5261.370519	24.974695
149.941834	5269.106675	24.979712
149.840232	5274.056432	24.984730
150.154315	5286.715856	24.989747
150.221311	5300.212628	24.994765
150.272837	5309.519817	24.999783
150.370210	5308.317692	25.004800
150.537824	5330.081741	25.009818
150.821057	5348.961470	25.014835
150.735908	5354.423204	25.019853
151.481509	5376.336664	25.024871
151.619414	5383.401764	25.029888
151.364343	5389.174229	25.034906
151.881300	5397.960302	25.039923
152.085349	5404.907722	25.044941
152.647493	5390.374834	25.049959
153.421475	5381.673826	25.054976
153.134349	5381.289530	25.059994
153.954080	5374.494288	25.065011
153.757955	5377.189251	25.070029
153.772070	5379.273611	25.075047
153.895736	5374.547698	25.080064
153.599022	5373.413621	25.085082
154.139677	5369.518870	25.090099
154.128731	5372.241641	25.095117
154.066764	5369.896515	25.100135
153.888722	5364.488685	25.105152
154.341106	5370.260793	25.110170
154.312075	5367.165538	25.115187
154.262514	5377.710222	25.120205
154.379888	5390.065930	25.125223
154.397807	5386.256227	25.130240
154.394187	5404.745335	25.135258
154.921055	5414.075965	25.140275
154.992606	5415.040188	25.145293
154.974109	5431.363031	25.150311
155.293823	5443.488207	25.155328
155.068003	5450.089466	25.160346
155.479535	5460.666131	25.165363
155.454338	5488.246742	25.170381
155.520954	5500.152760	25.175399
155.986212	5514.887845	25.180416
155.693945	5513.636266	25.185434
155.701504	5537.401715	25.190451
155.856051	5550.607168	25.195469
156.189112	5567.316991	25.200487
156.290513	5585.272132	25.205504
156.549957	5606.545465	25.210522
157.083459	5607.977121	25.215539
157.168065	5627.390169	25.220557
157.232591	5621.840091	25.225575
158.019825	5632.945141	25.230592
158.203864	5644.151011	25.235610
158.316839	5642.816995	25.240627
158.576442	5647.284112	25.245645
158.627451	5652.487852	25.250663
159.023907	5664.310736	25.255680
158.881040	5670.163568	25.260698
159.021343	5657.233870	25.265715
158.963826	5678.547474	25.270733
159.171227	5682.877569	25.275751
159.330159	5679.819105	25.280768
159.496972	5695.702781	25.285786
159.737742	5700.349637	25.290803
160.061665	5723.781662	25.295821
160.134923	5722.621168	25.300839
159.848442	5723.066977	25.305856
159.832396	5747.985440	25.310874
160.126495	5753.728804	25.315891
160.807922	5767.388513	25.320909
161.083042	5779.388316	25.325927
161.391954	5769.863478	25.330944
161.262273	5773.119455	25.335962
161.718032	5764.250309	25.340979
161.340906	5784.455592	25.345997
161.804634	5791.353007	25.351015
162.024531	5800.905547	25.356032
162.170518	5801.889696	25.361050
162.532396	5796.977989	25.366067
162.518274	5812.265082	25.371085
162.569018	5821.212787	25.376103
162.766332	5818.946939	25.381120
162.739988	5828.042464	25.386138
163.027138	5834.197318	25.391155
162.903946	5845.896542	25.396173
162.946560	5859.536442	25.401191
163.303186	5852.065433	25.406208
163.172539	5865.820871	25.411226
163.322502	5872.350783	25.416243
163.661432	5874.778905	25.421261
163.365320	5895.119984	25.426279
163.873160	5906.565707	25.431296
163.908440	5920.522476	25.436314
163.742450	5933.838400	25.441331
164.149496	5945.284154	25.446349
164.569309	5956.904694	25.451367
164.912443	5962.069071	25.456384
164.829255	5977.521802	25.461402
165.496265	5984.055985	25.466419
165.234917	5991.635284	25.471437
165.535861	6005.986131	25.476455
165.882561	6013.877403	25.481472
166.261230	6013.960159	25.486490
166.886742	6006.882596	25.491507
166.692591	6014.173583	25.496525
166.451950	6040.747048	25.501543
166.776563	6028.545838	25.506560
166.793202	6038.865871	25.511578
167.328924	6033.986845	25.516595
167.198670	6046.950009	25.521613
167.280833	6056.047589	25.526631
167.802357	6050.002779	25.531648
167.671961	6062.820766	25.536666
168.028040	6066.527874	25.541683
168.329621	6077.257864	25.546701
168.395894	6086.859875	25.551719
168.423831	6071.586224	25.556736
168.479330	6090.309834	25.561754
168.664464	6107.273771	25.566771
168.682618	6110.923342	25.571789
168.491265	6116.256730	25.576807
169.090160	6126.005764	25.581824
169.266532	6134.359408	25.586842
169.446666	6153.612837	25.591859
169.937728	6165.654827	25.596877
169.679496	6170.417859	25.601895
170.184644	6172.497989	25.606912
170.121686	6189.049448	25.611930
170.209068	6180.856543	25.616947
170.558194	6199.338544	25.621965
170.506458	6215.509453	25.626983
170.876591	6225.613216	25.632000
170.886417	6232.635574	25.637018
171.189049	6246.844289	25.642035
171.441747	6257.657806	25.647053
171.058123	6265.111161	25.652071
171.276300	6264.199416	25.657088
171.435463	6270.339742	25.662106
172.109728	6274.407431	25.667123
172.441917	6288.848309	25.672141
172.516926	6301.119722	25.677159
172.698241	6309.662081	25.682176
173.259868	6314.063105	25.687194
173.250019	6314.588704	25.692212
173.537867	6316.810225	25.697229
173.680776	6334.466016	25.702247
173.902460	6336.827334	25.707264
173.774561	6339.716941	25.712282
174.063734	6336.076052	25.717300
173.951615	6339.326221	25.722317
174.248569	6362.112985	25.727335
174.488531	6357.914730	25.732352
174.929023	6366.145025	25.737370
174.908614	6360.368111	25.742388
175.057112	6351.423704	25.747405
175.549090	6375.587873	25.752423
175.491555	6386.431127	25.757440
175.358981	6385.170252	25.762458
176.022208	6388.204258	25.767476
176.125597	6379.068024	25.772493
175.833490	6386.649148	25.777511
176.101938	6375.829725	25.782528
176.030823	6399.264524	25.787546
176.123719	6414.756330	25.792564
176.326116	6427.847589	25.797581
176.480291	6432.830195	25.802599
176.784543	6435.459549	25.807616
176.910396	6448.884810	25.812634
177.068159	6465.547154	25.817652
177.497815	6456.896430	25.822669
177.578925	6477.750445	25.827687
177.732718	6477.716906	25.832704
178.129970	6481.386082	25.837722
178.397555	6490.937826	25.842740
178.587304	6501.906564	25.847757
178.708431	6510.215368	25.852775
179.000555	6507.543134	25.857792
178.861099	6511.043850	25.862810
178.958276	6528.902716	25.867828
179.493735	6528.256937	25.872845
178.957368	6541.650266	25.877863
179.265375	6552.632077	25.882880
179.244994	6567.365173	25.887898
179.515925	6592.511314	25.892916
180.051753	6591.988593	25.897933
179.923674	6608.512749	25.902951
180.278486	6628.083409	25.907968
180.556868	6635.973026	25.912986
180.337941	6645.654735	25.918004
180.707489	6652.466213	25.923021
181.129600	6673.276498	25.928039
181.427987	6672.011225	25.933056
181.618665	6675.343448	25.938074
182.045490	6695.726842	25.943092
182.558620	6692.836860	25.948109
182.393701	6695.195654	25.953127
182.547432	6703.647811	25.958144
182.516187	6714.398747	25.963162
182.508051	6728.637581	25.968180
182.928522	6724.884497	25.973197
183.053240	6744.014638	25.978215
183.189970	6756.475571	25.983232
183.372000	6757.394145	25.988250
183.339244	6782.951165	25.993268
183.705409	6778.543631	25.998285
183.783810	6788.538721	26.003303
184.034957	6804.845798	26.008320
184.295779	6810.799908	26.013338
184.143520	6820.616482	26.018356
184.709607	6838.446386	26.023373
184.820120	6844.209385	26.028391
185.306123	6857.022909	26.033408
185.324383	6858.750058	26.038426
185.178821	6870.595498	26.043444
185.653539	6867.414758	26.048461
185.919041	6892.082311	26.053479
185.849122	6886.335086	26.058496
186.009438	6912.262966	26.063514
186.384126	6913.959537	26.068532
186.787992	6920.936213	26.073549
186.758798	6934.439786	26.078567
186.865541	6946.031079	26.083584
186.933167	6946.083648	26.088602
187.082651	6954.681805	26.093620
187.108033	6975.589311	26.098637
187.140572	6980.897344	26.103655
187.300381	6990.485174	26.108672
187.842673	6996.575195	26.113690
188.310994	7011.771921	26.118708
188.294834	7015.704857	26.123725
188.501648	7027.700396	26.128743
188.581659	7034.481610	26.133760
188.702997	7043.024235	26.138778
188.760755	7052.100877	26.143796
189.474111	7062.956353	26.148813
189.366624	7068.494705	26.153831
189.751116	7074.593688	26.158848
189.818316	7088.142255	26.163866
190.158031	7095.520508	26.168884
190.838853	7077.394042	26.173901
190.703719	7089.373738	26.178919
190.918492	7094.028180	26.183936
191.291889	7107.752936	26.188954
191.268925	7112.652984	26.193972
191.273247	7115.259972	26.198989
191.497182	7129.873163	26.204007
191.680406	7143.204707	26.209024
191.798793	7144.370043	26.214042
191.808332	7158.827427	26.219060
191.999610	7159.694063	26.224077
192.400660	7174.039613	26.229095
192.643781	7193.135888	26.234112
192.696299	7201.338946	26.239130
192.724730	7208.008339	26.244148
193.244116	7216.873837	26.249165
193.400978	7233.439152	26.254183
193.230763	7240.584809	26.259200
193.771990	7247.552719	26.264218
193.886737	7263.928927	26.269236
193.871301	7274.769266	26.274253
194.026308	7294.188833	26.279271
193.721205	7304.780969	26.284288
194.518972	7322.331961	26.289306
194.643634	7339.877925	26.294324
194.804524	7347.745215	26.299341
195.176182	7370.963506	26.304359
195.563504	7371.638433	26.309376
195.619551	7377.072334	26.314394
195.388565	7406.980041	26.319412
195.485544	7409.828272	26.324429
196.007049	7423.899430	26.329447
196.195431	7438.278504	26.334464
196.424073	7451.205373	26.339482
196.387289	7468.530504	26.344500
196.726699	7489.398868	26.349517
196.873952	7499.260434	26.354535
197.264025	7516.297748	26.359552
197.662037	7522.599969	26.364570
197.755211	7535.844879	26.369588
198.126268	7539.278440	26.374605
198.312067	7543.830196	26.379623
198.345832	7556.118380	26.384640
198.771791	7568.455626	26.389658
198.671175	7576.954345	26.394676
199.168945	7584.945754	26.399693
199.748464	7597.000087	26.404711
199.846421	7595.753525	26.409728
199.809219	7583.273325	26.414746
200.092132	7601.656615	26.419764
200.013140	7615.332654	26.424781
200.334086	7610.789942	26.429799
200.601189	7616.654933	26.434816
200.640188	7621.690634	26.439834
200.526466	7635.829898	26.444852
200.814675	7648.551838	26.449869
200.897758	7665.912046	26.454887
200.760886	7675.139452	26.459904
201.336674	7672.381573	26.464922
201.540757	7688.797833	26.469940
201.649324	7702.330900	26.474957
201.710509	7721.061592	26.479975
201.540787	7734.493054	26.484992
202.135805	7752.846543	26.490010
202.264205	7777.925078	26.495028
202.722578	7788.019038	26.500045
203.153500	7796.235692	26.505063
203.318333	7816.159400	26.510080
203.485203	7816.796268	26.515098
203.591501	7841.297451	26.520116
204.010045	7833.774904	26.525133
204.409565	7838.804698	26.530151
204.527329	7851.944956	26.535168
205.008350	7857.252439	26.540186
204.653228	7871.208705	26.545204
205.234889	7877.084486	26.550221
205.759586	7892.967668	26.555239
205.398652	7885.548269	26.560256
205.949469	7898.904857	26.565274
205.934309	7912.836311	26.570292
206.216064	7915.554646	26.575309
206.346755	7916.986457	26.580327
206.605431	7935.651701	26.585344
206.890032	7933.965455	26.590362
206.683946	7949.619046	26.595380
207.183456	7968.101368	26.600397
207.284605	7975.261624	26.605415
207.235175	7992.592384	26.610432
207.593664	7992.271053	26.615450
207.425026	8021.522781	26.620468
207.379116	8031.383320	26.625485
208.194917	8048.553331	26.630503
208.030888	8056.373954	26.635520
208.517492	8073.889171	26.640538
208.552418	8088.144407	26.645556
208.871053	8097.894203	26.650573
209.614053	8108.325760	26.655591
209.933087	8132.708761	26.660608
210.151767	8134.306760	26.665626
210.091904	8140.788266	26.670644
209.917991	8153.800791	26.675661
210.179919	8169.614877	26.680679
210.624728	8188.661644	26.685696
210.836799	8203.264916	26.690714
210.742809	8208.571023	26.695732
210.662654	8219.851425	26.700749
210.974927	8234.404296	26.705767
211.134606	8254.578697	26.710784
211.354902	8275.662354	26.715802
211.393181	8287.498843	26.720820
211.591220	8320.952594	26.725837
211.999877	8328.525758	26.730855
212.119173	8353.183440	26.735872
212.711386	8365.643563	26.740890
212.803769	8393.772080	26.745908
213.306908	8399.669802	26.750925
213.697259	8405.932484	26.755943
213.575727	8426.893062	26.760960
214.073199	8422.701359	26.765978
214.642974	8435.906980	26.770996
214.301186	8455.089876	26.776013
214.862922	8454.373623	26.781031
214.448130	8463.136654	26.786048
215.121486	8468.253167	26.791066
215.031671	8479.778343	26.796084
215.179162	8502.051292	26.801101
215.524191	8506.606757	26.806119
215.994244	8522.549556	26.811136
216.183269	8527.969278	26.816154
216.421457	8542.852874	26.821172
216.327577	8557.791660	26.826189
216.769905	8556.970979	26.831207
217.051451	8564.854616	26.836224
217.240959	8576.812830	26.841242
217.618059	8587.093606	26.846260
217.437984	8592.703772	26.851277
218.017507	8604.433574	26.856295
218.032550	8611.743325	26.861312
218.182410	8627.139665	26.866330
218.483032	8633.091289	26.871348
218.538916	8644.650572	26.876365
219.171634	8671.927661	26.881383
219.283860	8677.949857	26.886400
219.362773	8695.523217	26.891418
219.413326	8713.672493	26.896436
219.507737	8724.038675	26.901453
219.908830	8718.485456	26.906471
219.882156	8749.443091	26.911488
220.170434	8766.585909	26.916506
220.362350	8784.447902	26.921524
220.252758	8797.378184	26.926541
220.852793	8817.604188	26.931559
221.113310	8828.342218	26.936576
221.176119	8846.410773	26.941594
221.379282	8859.352091	26.946612
221.536922	8873.124591	26.951629
222.224564	8891.294212	26.956647
222.302492	8903.124883	26.961664
222.596237	8923.272695	26.966682
222.997835	8939.223421	26.971700
223.100774	8963.180407	26.976717
223.264112	8969.415699	26.981735
223.039461	8985.736096	26.986752
223.668205	8997.205856	26.991770
224.043835	8996.736591	26.996788
224.701861	9009.224727	27.001805
225.245805	9000.438103	27.006823
225.328838	9023.921538	27.011840
225.438662	9028.109848	27.016858
225.563323	9023.625959	27.021876
226.052297	9025.134335	27.026893
226.006463	9035.049069	27.031911
226.139984	9053.349858	27.036928
226.615323	9055.343437	27.041946
226.713900	9061.241605	27.046964
226.784477	9086.921381	27.051981
226.945340	9078.826188	27.056999
227.065221	9090.334678	27.062016
227.202417	9108.357105	27.067034
227.468184	9111.400167	27.072052
227.585027	9134.127010	27.077069
227.745744	9143.254852	27.082087
227.742643	9159.853266	27.087104
228.123773	9176.902985	27.092122
228.210726	9183.762832	27.097140
228.401690	9206.973849	27.102157
228.989880	9214.724478	27.107175
229.087047	9230.729461	27.112192
229.264569	9245.039022	27.117210
229.691654	9253.121165	27.122228
229.630059	9265.624330	27.127245
229.794812	9273.542352	27.132263
230.013182	9290.377717	27.137280
230.121753	9317.008526	27.142298
230.167558	9315.088038	27.147316
230.403445	9347.467376	27.152333
231.131135	9367.683456	27.157351
231.099431	9378.053972	27.162368
231.368449	9396.463323	27.167386
231.672059	9405.480503	27.172404
231.640118	9432.824947	27.177421
232.148778	9440.212406	27.182439
232.274980	9468.659301	27.187456
232.838499	9469.625603	27.192474
232.842061	9490.899303	27.197492
233.039180	9519.170982	27.202509
233.684882	9527.866256	27.207527
233.330917	9536.190858	27.212544
233.737855	9554.367216	27.217562
233.659691	9579.003782	27.222580
234.044785	9598.437080	27.227597
234.267842	9614.267960	27.232615
234.269048	9635.753738	27.237632
234.922769	9648.135630	27.242650
235.674809	9659.333896	27.247668
235.671655	9665.538671	27.252685
235.894934	9695.072630	27.257703
236.494363	9695.392370	27.262720
236.643110	9715.402729	27.267738
236.787250	9722.124362	27.272756
236.991065	9734.226321	27.277773
237.497060	9742.684676	27.282791
237.942614	9740.654161	27.287808
237.908956	9748.928679	27.292826
238.296818	9764.127648	27.297844
238.471832	9782.400552	27.302861
238.278254	9769.327687	27.307879
238.812677	9789.732373	27.312896
239.395009	9797.259990	27.317914
239.506332	9804.255174	27.322932
239.370873	9818.961521	27.327949
240.118916	9824.474023	27.332967
239.986093	9838.624268	27.337984
240.181001	9851.614931	27.343002
240.771489	9834.911306	27.348020
240.781535	9862.290848	27.353037
240.984721	9871.159801	27.358055
241.501163	9874.176351	27.363072
241.688717	9894.591287	27.368090
241.701414	9906.811705	27.373108
241.901570	9906.954034	27.378125
242.134228	9920.317722	27.383143
242.840112	9924.441276	27.388160
242.268284	9931.464590	27.393178
242.626890	9949.901501	27.398196
242.769150	9964.678124	27.403213
243.066988	9973.702800	27.408231
243.283751	9990.141213	27.413248
243.186130	10018.538758	27.418266
243.641013	10021.451307	27.423284
243.769980	10046.314953	27.428301
244.055070	10063.048998	27.433319
244.418997	10077.064772	27.438336
244.069764	10113.607059	27.443354
244.651416	10116.313474	27.448372
244.821338	10137.707093	27.453389
245.177995	10160.265006	27.458407
245.276382	10172.993157	27.463424
245.557066	10190.185839	27.468442
245.771208	10203.514742	27.473460
245.932703	10229.762823	27.478477
246.137380	10243.803670	27.483495
246.548879	10267.701365	27.488512
246.699559	10289.436023	27.493530
247.272455	10292.952154	27.498548
247.432058	10323.630621	27.503565
248.033757	10337.700910	27.508583
248.341745	10348.732345	27.513600
248.400837	10353.680386	27.518618
248.704374	10368.255244	27.523636
248.450741	10387.186341	27.528653
248.899347	10406.534753	27.533671
249.037846	10423.058430	27.538688
249.287780	10446.466990	27.543706
249.719924	10460.595509	27.548724
249.891876	10481.155618	27.553741
250.244666	10500.534925	27.558759
250.819847	10516.863976	27.563776
250.628970	10534.800243	27.568794
251.311006	10554.105926	27.573812
251.368325	10566.029291	27.578829
251.598833	10577.072999	27.583847
252.009522	10593.828893	27.588864
251.818040	10610.401270	27.593882
252.376719	10618.804409	27.598900
252.673039	10634.968850	27.603917
252.661227	10667.705035	27.608935
252.758404	10670.427435	27.613952
252.994196	10685.695184	27.618970
253.653002	10712.898559	27.623988
254.378684	10724.022661	27.629005
255.519934	10717.620355	27.634023
255.672452	10721.976024	27.639040
255.671282	10730.640582	27.644058
256.090146	10728.491000	27.649076
256.227993	10724.895072	27.654093
256.093295	10728.841047	27.659111
256.637615	10734.268907	27.664128
256.486026	10748.419621	27.669146
256.795187	10750.060513	27.674164
256.811535	10760.983158	27.679181
256.811413	10783.840847	27.684199
257.101052	10784.016530	27.689216
257.334958	10809.925695	27.694234
257.329962	10819.812875	27.699252
257.531762	10845.635548	27.704269
257.804872	10869.868294	27.709287
258.249622	10878.756721	27.714304
258.014859	10904.932048	27.719322
258.701255	10927.145576	27.724340
258.796774	10955.267991	27.729357
259.007371	10964.142618	27.734375
259.470656	10981.620027	27.739392
259.493584	10998.888565	27.744410
259.776524	11010.540049	27.749428
260.295403	11033.863006	27.754445
260.543043	11058.674671	27.759463
260.979464	11074.375479	27.764480
261.432076	11094.775464	27.769498
261.718286	11101.822677	27.774516
261.954564	11106.067429	27.779533
262.170091	11107.659869	27.784551
262.672611	11130.275043	27.789568
262.589278	11135.008779	27.794586
262.936443	11140.609738	27.799604
263.140909	11161.111820	27.804621
263.388149	11156.510334	27.809639
263.856267	11174.416604	27.814656
263.754122	11185.481205	27.819674
264.061262	11209.405925	27.824692
264.088693	11216.383203	27.829709
263.836025	11242.132364	27.834727
264.287958	11259.188685	27.839744
264.236956	11285.853610	27.844762
264.505480	11312.421153	27.849780
265.091727	11340.783038	27.854797
264.937288	11357.192387	27.859815
265.558875	11391.185249	27.864832
265.629624	11416.985031	27.869850
265.835312	11434.190604	27.874868
266.533194	11459.639589	27.879885
266.775484	11482.523307	27.884903
267.338744	11494.285906	27.889920
267.171680	11526.081653	27.894938
267.404604	11538.120224	27.899956
267.750241	11568.013735	27.904973
267.814114	11575.844332	27.909991
268.196318	11597.983159	27.915008
268.635607	11633.059691	27.920026
269.298552	11652.309503	27.925044
269.457282	11669.557383	27.930061
269.853237	11694.637165	27.935079
269.965345	11713.815443	27.940096
270.136993	11739.309349	27.945114
270.691946	11758.702496	27.950132
271.118031	11774.544450	27.955149
271.084382	11796.723392	27.960167
271.478002	11811.263158	27.965184
272.062361	11824.153131	27.970202
272.142337	11821.216556	27.975220
273.063875	11843.965889	27.980237
273.047150	11862.305593	27.985255
273.093744	11865.257133	27.990272
273.247317	11885.963759	27.995290
273.376810	11907.031007	28.000308
273.751634	11911.800531	28.005325
274.095783	11934.192020	28.010343
274.535328	11939.848218	28.015360
274.818594	11965.684931	28.020378
274.983126	11976.051404	28.025396
275.309066	11988.565147	28.030413
275.410526	12008.683252	28.035431
275.696501	12015.171920	28.040448
276.301845	12043.566611	28.045466
276.052221	12041.546866	28.050484
276.546827	12057.343589	28.055501
276.747960	12080.041856	28.060519
277.019437	12100.310261	28.065536
277.490268	12115.217102	28.070554
277.149388	12139.225571	28.075572
277.556871	12155.430749	28.080589
278.022729	12182.644377	28.085607
278.059358	12205.741186	28.090624
278.477556	12224.742564	28.095642
278.645859	12244.938869	28.100660
279.063026	12264.076235	28.105677
278.657112	12294.890717	28.110695
278.880506	12311.440649	28.115712
279.472466	12345.831449	28.120730
280.142780	12366.710281	28.125748
280.405960	12394.795950	28.130765
280.514850	12418.064853	28.135783
280.931201	12428.123711	28.140800
281.111780	12449.925656	28.145818
281.456721	12461.113597	28.150836
281.921764	12486.976232	28.155853
281.907710	12507.046647	28.160871
282.272135	12529.217775	28.165888
282.691509	12540.097264	28.170906
283.309082	12534.862700	28.175924
283.586909	12546.310677	28.180941
283.435834	12572.898359	28.185959
283.866888	12591.077047	28.190976
283.972465	12617.334063	28.195994
284.337260	12636.843168	28.201012
284.770614	12651.926830	28.206029
284.722615	12669.148009	28.211047
285.116889	12684.793607	28.216064
285.460983	12724.914444	28.221082
285.588705	12731.964993	28.226100
285.928026	12748.193990	28.231117
286.139311	12782.762060	28.236135
286.561856	12808.110738	28.241152
286.883113	12820.171028	28.246170
286.866204	12848.310720	28.251188
287.300034	12868.671360	28.256205
287.922414	12896.938351	28.261223
288.216170	12911.055658	28.266240
288.351662	12932.151530	28.271258
288.324663	12960.106650	28.276276
288.743502	12974.655995	28.281293
288.862327	13010.435823	28.286311
289.485692	13028.385857	28.291328
289.561906	13056.353372	28.296346
289.784759	13081.942122	28.301364
290.401704	13088.085626	28.306381
290.523411	13123.249414	28.311399
291.053686	13143.671034	28.316416
291.278352	13168.855398	28.321434
291.490807	13179.016073	28.326452
292.462222	13203.170852	28.331469
292.627983	13221.615921	28.336487
292.960097	13233.848463	28.341504
293.157817	13239.827155	28.346522
293.559781	13260.707961	28.351540
294.313585	13271.630224	28.356557
294.374673	13291.481272	28.361575
294.741440	13295.295541	28.366592
295.261351	13309.886156	28.371610
295.175038	13321.195849	28.376628
295.441376	13322.000496	28.381645
295.737301	13343.378019	28.386663
296.207915	13353.454136	28.391680
296.296610	13368.898688	28.396698
296.505176	13376.773684	28.401716
296.934764	13387.869965	28.406733
296.942568	13404.956749	28.411751
297.675441	13406.531507	28.416768
298.101264	13424.519178	28.421786
298.432772	13431.550697	28.426804
298.765074	13449.215134	28.431821
298.864011	13466.259275	28.436839
298.714075	13463.320566	28.441856
299.612359	13475.811958	28.446874
299.750435	13489.827763	28.451892
300.178514	13503.741306	28.456909
300.056610	13515.483023	28.461927
300.251368	13527.399363	28.466944
300.456836	13538.691901	28.471962
300.800924	13560.447404	28.476980
301.213098	13566.301023	28.481997
301.217735	13584.575886	28.487015
301.493854	13603.136677	28.492032
301.763334	13614.397126	28.497050
301.598027	13638.550519	28.502068
301.696275	13654.619100	28.507085
302.174183	13679.720261	28.512103
302.224785	13706.612691	28.517120
302.642335	13736.236249	28.522138
302.831460	13771.002233	28.527156
303.405031	13788.512344	28.532173
303.641000	13834.854922	28.537191
303.822324	13863.571416	28.542208
304.136144	13876.198842	28.547226
304.192843	13911.696397	28.552244
304.409624	13942.390739	28.557261
304.653181	13975.275817	28.562279
304.948457	14004.198898	28.567296
305.566054	14026.714251	28.572314
305.673077	14067.471945	28.577332
306.652857	14094.336221	28.582349
306.760087	14123.532115	28.587367
307.147520	14152.952603	28.592384
307.770645	14169.359430	28.597402
307.944229	14190.194923	28.602420
308.707804	14199.483437	28.607437
309.195186	14223.039500	28.612455
309.330546	14243.574699	28.617472
309.309185	14258.320312	28.622490
310.106699	14274.137762	28.627508
310.513846	14292.871348	28.632525
310.810251	14319.555599	28.637543
310.682635	14334.561094	28.642560
311.386659	14346.559240	28.647578
311.359903	14366.305159	28.652596
311.713479	14374.912656	28.657613
312.097759	14405.300428	28.662631
312.559097	14413.641567	28.667648
312.918912	14432.717472	28.672666
313.449465	14446.277730	28.677684
314.144026	14454.923437	28.682701
314.062813	14469.094326	28.687719
314.374161	14483.699567	28.692736
314.528060	14495.679762	28.697754
314.870673	14509.073697	28.702772
315.118084	14522.485712	28.707789
315.347610	14546.799478	28.712807
315.503433	14558.147771	28.717824
315.896458	14573.848816	28.722842
315.875922	14601.094737	28.727860
316.668394	14624.047661	28.732877
316.718327	14646.927436	28.737895
316.655544	14673.336834	28.742912
317.341112	14691.414505	28.747930
317.453213	14714.527805	28.752948
317.857956	14730.170295	28.757965
318.475646	14763.733994	28.762983
318.054040	14784.391761	28.768000
318.454399	14806.875745	28.773018
318.512793	14827.199393	28.778036
318.984279	14865.874107	28.783053
319.582520	14892.676107	28.788071
319.643791	14917.752575	28.793088
320.130753	14941.777016	28.798106
320.032399	14976.075431	28.803124
320.855129	14995.152025	28.808141
320.974482	15019.632090	28.813159
321.127599	15046.478766	28.818176
321.657932	15066.529769	28.823194
321.884417	15106.588777	28.828212
322.143928	15117.690605	28.833229
322.357993	15147.430346	28.838247
322.696232	15177.747602	28.843264
322.903514	15195.325861	28.848282
323.181458	15233.242059	28.853300
323.446890	15270.241221	28.858317
323.588019	15285.476978	28.863335
323.945732	15322.092262	28.868352
324.899441	15346.400988	28.873370
324.791345	15383.026188	28.878388
325.356458	15409.654077	28.883405
325.708249	15442.897411	28.888423
326.087350	15462.473501	28.893440
326.481649	15485.534052	28.898458
326.609533	15521.045551	28.903476
327.133485	15550.459440	28.908493
327.199323	15576.057183	28.913511
327.802523	15603.500552	28.918528
328.266677	15632.014321	28.923546
328.253945	15662.519973	28.928564
328.352945	15695.553831	28.933581
328.838072	15724.364499	28.938599
329.139747	15755.364292	28.943616
329.965831	15775.530789	28.948634
330.014152	15809.147610	28.953652
330.776323	15837.504458	28.958669
331.096256	15849.791126	28.963687
331.925350	15862.238083	28.968704
332.924148	15878.142201	28.973722
333.685461	15876.289000	28.978740
334.112645	15898.795333	28.983757
334.484925	15901.172186	28.988775
334.566205	15911.114826	28.993792
335.275170	15905.258626	28.998810
335.246767	15903.851286	29.003828
335.232544	15906.677169	29.008845
336.021421	15914.253857	29.013863
335.760887	15935.828838	29.018880
335.922929	15926.625094	29.023898
335.699774	15946.558167	29.028916
336.301503	15969.921602	29.033933
336.910329	15979.307877	29.038951
336.459994	15994.519984	29.043968
336.877789	16020.805421	29.048986
337.205748	16045.149889	29.054004
337.324393	16074.283801	29.059021
337.968534	16091.096432	29.064039
338.295847	16116.950833	29.069056
338.439996	16146.968386	29.074074
338.415160	16173.806612	29.079092
338.845824	16201.596869	29.084109
339.154406	16234.466168	29.089127
339.403781	16260.740413	29.094144
339.798012	16290.640054	29.099162
340.045665	16330.654081	29.104180
340.244637	16352.880844	29.109197
340.649018	16382.640064	29.114215
340.939867	16412.385529	29.119232
341.377707	16439.344318	29.124250
341.492899	16475.604976	29.129268
341.790763	16499.901039	29.134285
342.439500	16533.927278	29.139303
342.141523	16576.547787	29.144320
342.828526	16609.525851	29.149338
343.173144	16637.026995	29.154356
343.857520	16679.768647	29.159373
344.140551	16709.721100	29.164391
344.306781	16735.686845	29.169408
344.750398	16756.681816	29.174426
345.134681	16787.844053	29.179444
345.430607	16811.310108	29.184461
345.911789	16839.522938	29.189479
346.230898	16876.238827	29.194496
346.531459	16902.445915	29.199514
346.838535	16930.206045	29.204532
346.980040	16948.800643	29.209549
347.746646	16985.579303	29.214567
348.089407	17023.030878	29.219584
348.591161	17036.275308	29.224602
348.904111	17058.083887	29.229620
349.600668	17090.874920	29.234637
350.154601	17109.348214	29.239655
350.182666	17145.964908	29.244672
350.939911	17163.749413	29.249690
350.816854	17180.951658	29.254708
350.576561	17210.895263	29.259725
351.375644	17235.502252	29.264743
351.634540	17265.715198	29.269760
351.942223	17282.414169	29.274778
352.558975	17314.649526	29.279796
352.866296	17340.009631	29.284813
353.632219	17369.195720	29.289831
353.461467	17399.438272	29.294848
354.245541	17419.777331	29.299866
354.431007	17441.599994	29.304884
354.665680	17465.581827	29.309901
354.950601	17501.438780	29.314919
355.092226	17528.170685	29.319936
355.631072	17556.906190	29.324954
355.912172	17576.389227	29.329972
356.064852	17606.101316	29.334989
357.075075	17633.720728	29.340007
357.221560	17665.746051	29.345024
357.579940	17684.218939	29.350042
357.903602	17715.944943	29.355060
357.724057	17748.754294	29.360077
358.519254	17783.337841	29.365095
358.753440	17816.884818	29.370112
358.951506	17839.249258	29.375130
359.247754	17881.201504	29.380148
359.485011	17917.186724	29.385165
360.223636	17945.051284	29.390183
360.524199	17976.876094	29.395200
360.920728	18007.845693	29.400218
361.123777	18038.264435	29.405236
361.313490	18075.198708	29.410253
361.910898	18106.724532	29.415271
362.208706	18139.990445	29.420288
363.094429	18169.626478	29.425306
363.537588	18201.277698	29.430324
363.652914	18233.226708	29.435341
363.983785	18254.629500	29.440359
364.481617	18282.879732	29.445376
364.539458	18312.279241	29.450394
364.970946	18341.544453	29.455412
365.157423	18366.299382	29.460429
365.460990	18411.435721	29.465447
365.872593	18442.302568	29.470464
366.357787	18472.033390	29.475482
366.743225	18492.827718	29.480500
366.483188	18537.774653	29.485517
367.168005	18569.300171	29.490535
367.503159	18601.663908	29.495552
367.855401	18632.666711	29.500570
368.505226	18663.414464	29.505588
368.782967	18695.446192	29.510605
369.250074	18725.982590	29.515623
369.007213	18759.087859	29.520640
369.911404	18784.021514	29.525658
370.330136	18811.160339	29.530676
370.867907	18849.425157	29.535693
371.256301	18869.688729	29.540711
371.424674	18904.928427	29.545728
371.828431	18931.785464	29.550746
372.436115	18957.839818	29.555764
372.749441	18992.703171	29.560781
372.963122	19012.179255	29.565799
372.921018	19052.531746	29.570816
373.573359	19090.077807	29.575834
374.054271	19115.545713	29.580852
374.396438	19154.284021	29.585869
374.954201	19180.043232	29.590887
375.216200	19214.624397	29.595904
375.681725	19247.714301	29.600922
376.433012	19262.178438	29.605940
377.148113	19278.461504	29.610957
378.068883	19279.966284	29.615975
378.338046	19300.230026	29.620992
378.667400	19313.566201	29.626010
379.095585	19332.775241	29.631028
379.037546	19359.313488	29.636045
379.995813	19376.563105	29.641063
380.367899	19404.386085	29.646080
380.548744	19411.699281	29.651098
380.739543	19431.488949	29.656116
380.982621	19450.739736	29.661133
381.672267	19461.132252	29.666151
381.978124	19494.879386	29.671168
381.965765	19505.122847	29.676186
382.105894	19529.741198	29.681204
382.341234	19556.966649	29.686221
382.629952	19590.463910	29.691239
383.306662	19607.650428	29.696256
384.412122	19625.035160	29.701274
384.766193	19640.433691	29.706292
384.795619	19662.119015	29.711309
385.378013	19674.922992	29.716327
385.634980	19706.302555	29.721344
385.858632	19731.173435	29.726362
386.379980	19752.187906	29.731380
386.787175	19765.796511	29.736397
387.159607	19791.667696	29.741415
387.172221	19817.380461	29.746432
387.796921	19844.248372	29.751450
387.924773	19868.123532	29.756468
388.025792	19909.415726	29.761485
388.568029	19932.202517	29.766503
388.816005	19954.119294	29.771520
388.702365	19988.046712	29.776538
389.450087	20020.038587	29.781556
389.592850	20061.065515	29.786573
389.894679	20090.454752	29.791591
390.379317	20132.363374	29.796608
390.553256	20167.661337	29.801626
391.282505	20199.296259	29.806644
391.287363	20248.242979	29.811661
391.373962	20285.134398	29.816679
391.759467	20329.276679	29.821696
392.300935	20369.711064	29.826714
393.228779	20406.546761	29.831732
393.307452	20455.217064	29.836749
393.820131	20478.811548	29.841767
393.899076	20522.863278	29.846784
394.161931	20562.438178	29.851802
394.678479	20587.093669	29.856820
394.722907	20640.552796	29.861837
395.274673	20676.708656	29.866855
395.696710	20711.937143	29.871872
396.156461	20757.534625	29.876890
396.236965	20794.396360	29.881908
396.602832	20851.881098	29.886925
397.018223	20889.682552	29.891943
397.625024	20930.752340	29.896960
398.237965	20979.062238	29.901978
398.701812	21015.624238	29.906996
398.678059	21067.528213	29.912013
399.505286	21102.750798	29.917031
399.933325	21138.648872	29.922048
400.288436	21183.770884	29.927066
400.995105	21225.678648	29.932084
401.419491	21262.885463	29.937101
401.924437	21294.696292	29.942119
402.474666	21331.182161	29.947136
402.503762	21371.553531	29.952154
403.060250	21406.035558	29.957172
403.533276	21442.925481	29.962189
403.731993	21480.389207	29.967207
404.423521	21519.999980	29.972224
404.653561	21554.451257	29.977242
405.064917	21583.414851	29.982260
405.761303	21613.534394	29.987277
406.045888	21657.733369	29.992295
406.901997	21687.809050	29.997312
406.846040	21719.822157	30.002330
407.360436	21757.432842	30.007348
407.797090	21792.654650	30.012365
408.364327	21828.835474	30.017383
408.984564	21867.990524	30.022400
409.647329	21901.458403	30.027418
409.927990	21920.269725	30.032436
410.415917	21952.059003	30.037453
410.654644	21977.088327	30.042471
411.127280	22011.578226	30.047488
411.440956	22044.589203	30.052506
411.782071	22063.909336	30.057524
412.208198	22111.410860	30.062541
412.396569	22138.053263	30.067559
413.162335	22167.613043	30.072576
413.125629	22205.096058	30.077594
413.700387	22226.054256	30.082612
414.159327	22267.573349	30.087629
414.768268	22299.754958	30.092647
414.836453	22334.030737	30.097664
415.236372	22367.249905	30.102682
416.032877	22398.208017	30.107700
416.145258	22436.761293	30.112717
416.807184	22466.167172	30.117735
417.267930	22508.166727	30.122752
417.242846	22533.560343	30.127770
417.917616	22570.749356	30.132788
418.406487	22608.201359	30.137805
418.591358	22640.784853	30.142823
418.795923	22676.240474	30.147840
419.451196	22705.243332	30.152858
419.760955	22745.687278	30.157876
419.953060	22783.969659	30.162893
420.269196	22816.810919	30.167911
420.884362	22853.744396	30.172928
421.357816	22895.660631	30.177946
421.644169	22919.641032	30.182964
422.238992	22962.947559	30.187981
422.490295	22990.529116	30.192999
423.150024	23017.079910	30.198016
423.997161	23043.373895	30.203034
424.568577	23071.297211	30.208052
424.858272	23104.263151	30.213069
425.257847	23127.916430	30.218087
425.802954	23152.261010	30.223104
425.984382	23174.798423	30.228122
427.083484	23211.618850	30.233140
427.555597	23232.865916	30.238157
427.483087	23264.511268	30.243175
427.756060	23290.813365	30.248192
427.716623	23328.393709	30.253210
428.481432	23352.053239	30.258228
428.286745	23393.575955	30.263245
429.039710	23432.991349	30.268263
429.219517	23466.499600	30.273280
429.272557	23517.778656	30.278298
429.962050	23559.719323	30.283316
430.315397	23602.053973	30.288333
430.408970	23654.003197	30.293351
430.995194	23688.604601	30.298368
431.198603	23739.058114	30.303386
431.681596	23779.969935	30.308404
432.191154	23828.252409	30.313421
432.649327	23883.841967	30.318439
432.924567	23922.359966	30.323456
433.343634	23977.431397	30.328474
433.762555	24031.081124	30.333492
434.344230	24083.814457	30.338509
434.719930	24137.882006	30.343527
435.708148	24185.256195	30.348544
435.906859	24230.959415	30.353562
436.641486	24264.420015	30.358580
437.286556	24297.648237	30.363597
437.845338	24337.835219	30.368615
437.852194	24388.378029	30.373632
438.315244	24438.963264	30.378650
438.831153	24473.722390	30.383668
439.878847	24500.448217	30.388685
440.154139	24538.455503	30.393703
440.817580	24573.798378	30.398720
441.778629	24603.918917	30.403738
442.761032	24620.948171	30.408756
444.010252	24629.555795	30.413773
444.422116	24646.307895	30.418791
445.081279	24653.333243	30.423808
445.352811	24654.681062	30.428826
445.742250	24674.236305	30.433844
446.168394	24683.889223	30.438861
445.860884	24693.783452	30.443879
446.434129	24713.891353	30.448896
446.752973	24741.193000	30.453914
447.113595	24759.602658	30.458932
447.410076	24777.997101	30.463949
447.489587	24805.955652	30.468967
448.035783	24828.677943	30.473984
448.163674	24863.719711	30.479002
448.321777	24890.256772	30.484020
449.139595	24929.715518	30.489037
449.049131	24968.077934	30.494055
449.202387	25005.169895	30.499072
449.451718	25050.930250	30.504090
450.048625	25085.526075	30.509108
450.201995	25126.681867	30.514125
450.249278	25175.760449	30.519143
450.718508	25200.530197	30.524160
451.250176	25254.045456	30.529178
452.126124	25289.697579	30.534196
452.833827	25324.996925	30.539213
453.330619	25368.033298	30.544231
453.670575	25403.769576	30.549248
454.259245	25438.133462	30.554266
454.654913	25474.019135	30.559284
455.262369	25512.867343	30.564301
455.767437	25545.373810	30.569319
456.234127	25575.250924	30.574336
456.515317	25610.952533	30.579354
457.340957	25656.725115	30.584372
457.506620	25686.611624	30.589389
457.405155	25732.807669	30.594407
458.099807	25765.069916	30.599424
458.825115	25817.128019	30.604442
458.714613	25861.657289	30.609460
459.411525	25899.708547	30.614477
459.580781	25950.305677	30.619495
460.493013	25975.259793	30.624512
461.111655	26024.389987	30.629530
461.323688	26064.963375	30.634548
461.934509	26110.859115	30.639565
462.252999	26156.946109	30.644583
463.012732	26196.403795	30.649600
462.892076	26245.789364	30.654618
463.223684	26293.536815	30.659636
463.841899	26342.680488	30.664653
464.094420	26393.689136	30.669671
464.908685	26445.115544	30.674688
465.420401	26495.704638	30.679706
465.954856	26540.728481	30.684724
466.352213	26578.436080	30.689741
466.945495	26633.266274	30.694759
467.485064	26676.652668	30.699776
467.772484	26718.384808	30.704794
467.929435	26783.737527	30.709812
468.682023	26825.087332	30.714829
468.969164	26873.816444	30.719847
469.573719	26917.275338	30.724864
470.306822	26974.005942	30.729882
470.474283	27019.631881	30.734900
470.929748	27059.587653	30.739917
471.519966	27116.284150	30.744935
472.077415	27154.410173	30.749952
472.493933	27210.900284	30.754970
472.514937	27259.766811	30.759988
473.280883	27304.048196	30.765005
473.910705	27359.658366	30.770023
474.343393	27401.413397	30.775040
474.619916	27464.531073	30.780058
474.869088	27510.682559	30.785076
475.989452	27547.823634	30.790093
476.229511	27604.051727	30.795111
476.920988	27647.523849	30.800128
477.586340	27692.182108	30.805146
477.712807	27733.979462	30.810164
478.433398	27784.469519	30.815181
478.717516	27847.858978	30.820199
479.242303	27881.826171	30.825216
479.990643	27924.468292	30.830234
480.313308	27977.720080	30.835252
481.022106	28028.642395	30.840269
481.312598	28069.422394	30.845287
482.143354	28106.900603	30.850304
482.137708	28150.704211	30.855322
482.720388	28193.366519	30.860340
483.749639	28225.276875	30.865357
484.156195	28263.978514	30.870375
484.561200	28296.770532	30.875392
485.073108	28335.070237	30.880410
485.031779	28363.975450	30.885428
485.755735	28407.791748	30.890445
486.012654	28453.931509	30.895463
486.586848	28498.138066	30.900480
486.896493	28540.116964	30.905498
487.402032	28594.169746	30.910516
487.885227	28624.674526	30.915533
488.231207	28678.537612	30.920551
488.895440	28718.647238	30.925568
489.462087	28755.219865	30.930586
489.498384	28813.853544	30.935604
490.264550	28859.124336	30.940621
490.477283	28914.677644	30.945639
491.146767	28970.911762	30.950656
491.428162	29022.194256	30.955674
492.283893	29068.184719	30.960692
493.114961	29103.420742	30.965709
493.393482	29160.026343	30.970727
493.566009	29195.567942	30.975744
493.966065	29247.312813	30.980762
494.660380	29305.414997	30.985780
495.638697	29335.887534	30.990797
496.187164	29387.400917	30.995815
496.639222	29424.428841	31.000832
497.404234	29468.632887	31.005850
497.929754	29510.681095	31.010868
498.986346	29541.729546	31.015885
499.792333	29576.110631	31.020903
499.759445	29615.597939	31.025920
500.187488	29646.163445	31.030938
500.865223	29692.404426	31.035956
501.588048	29717.576120	31.040973
502.100405	29760.221095	31.045991
502.516787	29796.522014	31.051008
503.058165	29822.335416	31.056026
503.377088	29855.257188	31.061044
504.195059	29889.314535	31.066061
504.316647	29933.184186	31.071079
504.269089	29979.691121	31.076096
504.774204	30013.658606	31.081114
505.155474	30066.969842	31.086132
505.616099	30110.514951	31.091149
505.860015	30157.823695	31.096167
506.224908	30199.683540	31.101184
506.701107	30255.009554	31.106202
506.785513	30313.583067	31.111220
507.513673	30373.629954	31.116237
508.221379	30428.660994	31.121255
508.895580	30482.888282	31.126272
509.190989	30536.245782	31.131290
509.257842	30605.461913	31.136308
509.817737	30656.521525	31.141325
510.130741	30705.167179	31.146343
510.607333	30762.732307	31.151360
511.049935	30833.767846	31.156378
511.551285	30899.338899	31.161396
512.530714	30953.089744	31.166413
513.172023	31009.175789	31.171431
513.605658	31082.704302	31.176448
514.258083	31127.296186	31.181466
515.335372	31174.653731	31.186484
516.346583	31207.804274	31.191501
516.929024	31253.305069	31.196519
517.557470	31287.501873	31.201536
518.384809	31314.966568	31.206554
518.556101	31351.738476	31.211572
519.091339	31382.201254	31.216589
519.658655	31411.609644	31.221607
519.924051	31445.617023	31.226624
520.380069	31492.870303	31.231642
520.650906	31520.719554	31.236660
521.260260	31563.934654	31.241677
521.665484	31612.334083	31.246695
521.998224	31644.301941	31.251712
522.813955	31679.140169	31.256730
523.007778	31740.399984	31.261748
523.797398	31780.249369	31.266765
524.380786	31817.893191	31.271783
524.920144	31852.597984	31.276800
525.224769	31898.737959	31.281818
525.768225	31953.153933	31.286836
526.260174	32003.696456	31.291853
526.577297	32048.456627	31.296871
527.152277	32105.080736	31.301888
527.753911	32135.445710	31.306906
528.124885	32191.849128	31.311924
528.665587	32249.642242	31.316941
529.184911	32306.838272	31.321959
529.698976	32353.951650	31.326976
530.569113	32399.384601	31.331994
530.585038	32445.128457	31.337012
531.585366	32492.052190	31.342029
532.568488	32526.176513	31.347047
532.872152	32569.112826	31.352064
534.216214	32615.888171	31.357082
534.299025	32667.811378	31.362100
534.961387	32710.704446	31.367117
534.965153	32761.021798	31.372135
535.365360	32804.493500	31.377152
535.797561	32848.801130	31.382170
536.045830	32911.099004	31.387188
536.288784	32959.558578	31.392205
536.985101	33022.564242	31.397223
537.547383	33081.468983	31.402240
538.175234	33127.725422	31.407258
538.364047	33190.027113	31.412276
539.152209	33242.795933	31.417293
539.681234	33292.671921	31.422311
539.834879	33360.916274	31.427328
540.433238	33419.380072	31.432346
540.729410	33476.898750	31.437364
541.386112	33547.043817	31.442381
542.187971	33610.654308	31.447399
542.731128	33674.356088	31.452416
543.713434	33729.118897	31.457434
543.913562	33797.995952	31.462452
544.887512	33839.862546	31.467469
545.606531	33888.009443	31.472487
546.303998	33939.769974	31.477504
547.212001	33994.203697	31.482522
547.529028	34053.826081	31.487540
547.835875	34090.878723	31.492557
548.315360	34146.720333	31.497575
548.800526	34207.088169	31.502592
549.489678	34247.596566	31.507610
549.795282	34305.172928	31.512628
550.063537	34360.169342	31.517645
550.716182	34418.747539	31.522663
550.978100	34485.562299	31.527680
551.692260	34541.330261	31.532698
551.967700	34601.283159	31.537716
552.387145	34651.862375	31.542733
552.838162	34724.737048	31.547751
553.356248	34778.538359	31.552768
553.737711	34836.395131	31.557786
554.058591	34904.649891	31.562804
554.707454	34969.104076	31.567821
555.554513	35033.881494	31.572839
555.723446	35105.499151	31.577856
556.781818	35157.680354	31.582874
557.820172	35207.405220	31.587892
558.509444	35267.491196	31.592909
559.280920	35318.168617	31.597927
560.122536	35365.534606	31.602944
560.756674	35409.676881	31.607962
560.812340	35468.692917	31.612980
561.585328	35514.647322	31.617997
562.111665	35573.893436	31.623015
562.494774	35632.789090	31.628032
563.396794	35681.316080	31.633050
563.674842	35745.963482	31.638068
563.945749	35789.689206	31.643085
564.873833	35836.334521	31.648103
565.357280	35905.812678	31.653120
565.784744	35950.291952	31.658138
565.834169	36013.635474	31.663156
566.423496	36079.600930	31.668173
567.271484	36135.326827	31.673191
567.436867	36198.184822	31.678208
568.498142	36264.013701	31.683226
569.172773	36330.276408	31.688244
569.671061	36394.998777	31.693261
570.191096	36459.597795	31.698279
570.570797	36525.774510	31.703296
571.060039	36582.405078	31.708314
572.232582	36636.993849	31.713332
573.357827	36681.852258	31.718349
575.025142	36717.330571	31.723367
575.779837	36750.182253	31.728384
576.559053	36782.947942	31.733402
576.778743	36828.239357	31.738420
577.716352	36853.385993	31.743437
578.341748	36884.215684	31.748455
578.683781	36918.845890	31.753472
579.218351	36953.136151	31.758490
579.784903	36991.740346	31.763508
580.001447	37029.590029	31.768525
580.340144	37079.485757	31.773543
580.374641	37125.034447	31.778560
581.047683	37167.081205	31.783578
581.443929	37225.119200	31.788596
581.567775	37276.610933	31.793613
582.432758	37328.973184	31.798631
582.590532	37390.760873	31.803648
583.258213	37452.133732	31.808666
583.702589	37515.261749	31.813684
584.086292	37577.786066	31.818701
584.717799	37628.642660	31.823719
585.318490	37700.770512	31.828736
586.007324	37763.658616	31.833754
586.278345	37823.969052	31.838772
586.838234	37889.255411	31.843789
587.332446	37951.921598	31.848807
587.689539	38033.757640	31.853824
588.563748	38087.049878	31.858842
589.001656	38145.962828	31.863860
590.083053	38224.612817	31.868877
590.703219	38279.298604	31.873895
591.068459	38338.843193	31.878912
592.105540	38399.224975	31.883930
592.426192	38450.043658	31.888948
592.843182	38504.863018	31.893965
593.715768	38554.147343	31.898983
594.118159	38623.571103	31.904000
594.467039	38673.336125	31.909018
595.099679	38734.882545	31.914036
595.329488	38805.073814	31.919053
596.212840	38869.351237	31.924071
597.141496	38929.776779	31.929088
597.333618	38996.331960	31.934106
597.932815	39049.631700	31.939124
598.746335	39118.328636	31.944141
599.304204	39184.295893	31.949159
599.839248	39251.253480	31.954176
600.157560	39312.363815	31.959194
601.215555	39372.245436	31.964212
601.678854	39447.859918	31.969229
602.426244	39502.408712	31.974247
603.200959	39578.752747	31.979264
603.563763	39638.927380	31.984282
604.108748	39711.367895	31.989300
604.747232	39771.170860	31.994317
605.704093	39830.241109	31.999335
606.241335	39901.861320	32.004352
606.358861	39954.865585	32.009370
607.238751	40023.169206	32.014388
607.568407	40100.267796	32.019405
608.375405	40169.209398	32.024423
608.812822	40245.950111	32.029440
609.221627	40315.928489	32.034458
610.061804	40389.817581	32.039476
610.343375	40474.628142	32.044493
610.987085	40547.214081	32.049511
611.348693	40631.715467	32.054528
612.052814	40703.735911	32.059546
612.885820	40780.827639	32.064564
613.250212	40864.064583	32.069581
613.833536	40945.351214	32.074599
614.496745	41032.646640	32.079616
615.272926	41108.312739	32.084634
616.494168	41169.565145	32.089652
617.261012	41239.869880	32.094669
618.021047	41305.331214	32.099687
618.839538	41370.277614	32.104704
619.364330	41436.383350	32.109722
620.238269	41496.097236	32.114740
620.945374	41554.060162	32.119757
621.795286	41614.170265	32.124775
622.514580	41677.830211	32.129792
623.156838	41735.797448	32.134810
624.009180	41794.073475	32.139828
624.562711	41855.988952	32.144845
625.397849	41902.731490	32.149863
625.662789	41956.862302	32.154880
626.149922	42007.271053	32.159898
626.731755	42063.705349	32.164916
627.051065	42126.354004	32.169933
627.748305	42186.489582	32.174951
628.320539	42241.515380	32.179968
628.613475	42319.550954	32.184986
629.203512	42375.915190	32.190004
629.848960	42447.305389	32.195021
630.436021	42509.628574	32.200039
630.973078	42585.634478	32.205056
631.399957	42653.068478	32.210074
632.287956	42721.714457	32.215092
632.700099	42797.152419	32.220109
633.288767	42860.576907	32.225127
633.758384	42929.738136	32.230144
634.581435	42993.006119	32.235162
635.219829	43051.913538	32.240180
636.088431	43120.304460	32.245197
637.009362	43164.797120	32.250215
637.435731	43236.717541	32.255232
637.739594	43295.077101	32.260250
638.481599	43352.957057	32.265268
639.117007	43423.877583	32.270285
639.583244	43496.823621	32.275303
639.951835	43583.802083	32.280320
640.689873	43654.359379	32.285338
641.453829	43721.623656	32.290356
641.887314	43793.506811	32.295373
642.421150	43863.995546	32.300391
642.916595	43947.697985	32.305408
643.126383	44031.432823	32.310426
643.837744	44109.839289	32.315444
644.483541	44205.980318	32.320461
645.555915	44289.157228	32.325479
646.005471	44371.445201	32.330496
646.231377	44450.871396	32.335514
647.261129	44533.404358	32.340532
647.491657	44628.075120	32.345549
648.600764	44711.273150	32.350567
649.466095	44803.087261	32.355584
650.323576	44883.118229	32.360602
650.925609	44951.284514	32.365620
651.916830	45038.765748	32.370637
652.423386	45114.905247	32.375655
652.999812	45190.483722	32.380672
653.739862	45266.574518	32.385690
655.291907	45332.119798	32.390708
655.845669	45403.217541	32.395725
657.026703	45460.793825	32.400743
657.654450	45520.961948	32.405760
658.256472	45589.199757	32.410778
659.244473	45659.142253	32.415796
659.696217	45730.680843	32.420813
660.060555	45789.309455	32.425831
660.709894	45849.702809	32.430848
661.201799	45913.524354	32.435866
661.750846	45979.911808	32.440884
662.672930	46057.147080	32.445901
663.685200	46113.397701	32.450919
664.122750	46182.415863	32.455936
664.679058	46249.334361	32.460954
665.519222	46313.020258	32.465972
665.509534	46377.396123	32.470989
665.958719	46451.935973	32.476007
667.160822	46535.379241	32.481024
667.898571	46609.311392	32.486042
668.107490	46679.815569	32.491060
668.439877	46748.681121	32.496077
668.864187	46830.456968	32.501095
669.849008	46910.310717	32.506112
670.365992	46996.627551	32.511130
671.097691	47072.377802	32.516148
672.032983	47152.505867	32.521165
672.499167	47245.063025	32.526183
673.411452	47311.505050	32.531200
674.112460	47390.234559	32.536218
674.785726	47466.026907	32.541236
675.179178	47549.404430	32.546253
676.015021	47629.992603	32.551271
676.777577	47710.662130	32.556288
677.151077	47779.821713	32.561306
678.014334	47852.428675	32.566324
678.371748	47914.239779	32.571341
679.171347	47989.583882	32.576359
679.843555	48067.959632	32.581376
680.239533	48149.744659	32.586394
680.983794	48219.783849	32.591412
681.596051	48295.202586	32.596429
682.023002	48383.360848	32.601447
682.951146	48457.275519	32.606464
683.302247	48543.333164	32.611482
684.118829	48619.125881	32.616500
685.019600	48704.414765	32.621517
685.586205	48789.534862	32.626535
686.636695	48867.980650	32.631552
687.134170	48948.303800	32.636570
687.897891	49032.324697	32.641588
688.920089	49106.372253	32.646605
689.249471	49187.772824	32.651623
690.454636	49267.113154	32.656640
691.022363	49348.306141	32.661658
691.827827	49408.595920	32.666676
692.638581	49493.110967	32.671693
693.406531	49575.595737	32.676711
694.028649	49648.562511	32.681728
694.583437	49732.884424	32.686746
695.391146	49802.032729	32.691764
695.933454	49878.239524	32.696781
696.697875	49965.661360	32.701799
697.105579	50042.547796	32.706816
697.803228	50135.055078	32.711834
698.463596	50219.634303	32.716852
698.832511	50299.773504	32.721869
699.771636	50389.706788	32.726887
700.290694	50464.318374	32.731904
701.161244	50555.212125	32.736922
701.714904	50641.834327	32.741940
702.472957	50738.175221	32.746957
703.150042	50822.867925	32.751975
704.279147	50905.845039	32.756992
705.313620	50993.766296	32.762010
706.122950	51070.510994	32.767028
706.615410	51146.362783	32.772045
707.160319	51231.615508	32.777063
708.250741	51309.936803	32.782080
708.959689	51402.706803	32.787098
709.472876	51481.808769	32.792116
710.445859	51562.572743	32.797133
710.981230	51639.855771	32.802151
711.496933	51707.062314	32.807168
712.305794	51799.837233	32.812186
712.956854	51884.234154	32.817204
713.943681	51976.020106	32.822221
714.208101	52056.814495	32.827239
714.810332	52140.909935	32.832256
715.358335	52232.917481	32.837274
716.265114	52319.819671	32.842292
716.862806	52421.602859	32.847309
717.434574	52512.070134	32.852327
717.977944	52601.327266	32.857344
718.974202	52697.082110	32.862362
719.628506	52788.360146	32.867380
720.220602	52871.706783	32.872397
720.625083	52976.635955	32.877415
721.567483	53055.517833	32.882432
722.394883	53157.287224	32.887450
723.029681	53251.506289	32.892468
723.490167	53347.999472	32.897485
724.024702	53449.379356	32.902503
725.092422	53546.233878	32.907520
725.616271	53638.054543	32.912538
726.569960	53714.177814	32.917556
728.136388	53779.675371	32.922573
729.399525	53861.756055	32.927591
730.372499	53926.423045	32.932608
731.054974	54002.266983	32.937626
731.960117	54063.375872	32.942644
732.953506	54130.641117	32.947661
733.568816	54201.598170	32.952679
734.068129	54255.303786	32.957696
734.631939	54334.293531	32.962714
734.868311	54399.912500	32.967732
735.681603	54471.573441	32.972749
736.683096	54548.027317	32.977767
737.494835	54619.372533	32.982784
738.334085	54698.016596	32.987802
738.983075	54778.576577	32.992820
739.499700	54851.405251	32.997837
740.103252	54929.593376	33.002855
740.874252	55008.527608	33.007872
741.125572	55099.276482	33.012890
741.825827	55181.329650	33.017908
742.762267	55270.630248	33.022925
743.210412	55368.272733	33.027943
744.064126	55452.853213	33.032960
744.329141	55544.158552	33.037978
745.014507	55638.822199	33.042996
745.902472	55727.119519	33.048013
746.522302	55826.084994	33.053031
747.121627	55925.237623	33.058048
747.895244	56026.932831	33.063066
748.951955	56128.033540	33.068084
749.854853	56220.026335	33.073101
750.257608	56320.382207	33.078119
750.727281	56426.582188	33.083136
751.974295	56516.294486	33.088154
752.586964	56605.986207	33.093172
754.122293	56702.742400	33.098189
754.484139	56803.277578	33.103207
754.667120	56902.670329	33.108224
755.564807	57004.711007	33.113242
756.372948	57100.614343	33.118260
757.305280	57206.017482	33.123277
758.067086	57301.340273	33.128295
759.114954	57395.314854	33.133312
759.664728	57493.513368	33.138330
760.456230	57593.503549	33.143348
761.527252	57694.925069	33.148365
761.889015	57793.939063	33.153383
762.940275	57885.471954	33.158400
763.668831	57990.606629	33.163418
764.104409	58088.565944	33.168436
765.323693	58178.041936	33.173453
765.494644	58294.214923	33.178471
766.306751	58382.704765	33.183488
767.609786	58475.346072	33.188506
768.699615	58569.324975	33.193524
769.734907	58643.875149	33.198541
770.802662	58740.763374	33.203559
771.791647	58811.238827	33.208576
772.383525	58898.378886	33.213594
772.750898	58991.377554	33.218612
773.909559	59082.290514	33.223629
774.797903	59164.954435	33.228647
775.279198	59249.764805	33.233664
775.734462	59343.225770	33.238682
776.212530	59431.917320	33.243700
777.143234	59508.974063	33.248717
777.280464	59600.631232	33.253735
777.974075	59687.226487	33.258752
778.557885	59795.271634	33.263770
779.027691	59892.764448	33.268788
779.736176	59990.891230	33.273805
780.458587	60093.839523	33.278823
781.311185	60205.933434	33.283840
781.883846	60305.779136	33.288858
782.495626	60414.221410	33.293876
783.709127	60522.816805	33.298893
784.322699	60631.126828	33.303911
785.244425	60725.792336	33.308928
786.033328	60831.638756	33.313946
786.952968	60948.118558	33.318964
787.851148	61051.214246	33.323981
788.582204	61158.862530	33.328999
789.843422	61252.919857	33.334016
790.697210	61351.978829	33.339034
791.435898	61463.298710	33.344052
792.667833	61550.189709	33.349069
793.295193	61651.190716	33.354087
793.859827	61740.946841	33.359104
794.767256	61851.836912	33.364122
796.008863	61940.063447	33.369140
796.997328	62038.072245	33.374157
797.608200	62140.698383	33.379175
798.660455	62222.485996	33.384192
799.829957	62303.654135	33.389210
800.531940	62397.322278	33.394228
802.174078	62467.832555	33.399245
803.249992	62549.642864	33.404263
803.926858	62621.349248	33.409280
804.785361	62698.212038	33.414298
805.285752	62786.696921	33.419316
805.863921	62865.363997	33.424333
806.302410	62944.388711	33.429351
807.144250	63036.973833	33.434368
807.935162	63122.654299	33.439386
808.393314	63219.541657	33.444404
809.261918	63311.496878	33.449421
810.001144	63403.409390	33.454439
810.709865	63495.719518	33.459456
811.576090	63592.886276	33.464474
812.436442	63684.179438	33.469492
813.066354	63777.205652	33.474509
813.863923	63869.401951	33.479527
814.936905	63962.372134	33.484544
815.738019	64069.851108	33.489562
816.390900	64168.553904	33.494580
817.170495	64265.344321	33.499597
817.693359	64371.291773	33.504615
818.663676	64464.558448	33.509632
819.299819	64565.804113	33.514650
819.995776	64669.959388	33.519668
821.226201	64757.241654	33.524685
822.281723	64858.562107	33.529703
823.279786	64953.136762	33.534720
824.415184	65046.069519	33.539738
824.921068	65143.456968	33.544756
825.925173	65231.567698	33.549773
826.922012	65318.742868	33.554791
827.795179	65408.197919	33.559808
828.218594	65505.441395	33.564826
829.111514	65597.109926	33.569844
829.690430	65680.027583	33.574861
830.213217	65788.355185	33.579879
831.193267	65881.207702	33.584896
832.177769	65976.345452	33.589914
832.469139	66068.540407	33.594932
833.456702	66158.860242	33.599949
834.114780	66252.030445	33.604967
834.393001	66352.902433	33.609984
835.466197	66450.414994	33.615002
835.929054	66550.505415	33.620020
836.954321	66654.889524	33.625037
837.598818	66767.077074	33.630055
838.586795	66874.253766	33.635072
839.379816	66978.352656	33.640090
839.994487	67093.883024	33.645108
840.472666	67205.921256	33.650125
841.390754	67314.883580	33.655143
841.924927	67438.348948	33.660160
842.504426	67555.013931	33.665178
843.368307	67690.281767	33.670196
844.223093	67801.611461	33.675213
845.251295	67938.919018	33.680231
846.285028	68069.907309	33.685248
847.351929	68182.300835	33.690266
847.935742	68326.062516	33.695284
848.517953	68433.473877	33.700301
849.690794	68552.887152	33.705319
850.307860	68677.890463	33.710336
851.512450	68805.208530	33.715354
852.367051	68940.636339	33.720372
853.353385	69061.151272	33.725389
854.394143	69198.393900	33.730407
854.824369	69317.838334	33.735424
856.053043	69443.921006	33.740442
856.821797	69563.167919	33.745460
857.686257	69686.668287	33.750477
858.743845	69815.673361	33.755495
859.863791	69940.812967	33.760512
860.582192	70065.762758	33.765530
861.594784	70191.047020	33.770548
862.466181	70305.019101	33.775565
863.362061	70434.970745	33.780583
864.056238	70552.492452	33.785600
865.408088	70667.150768	33.790618
865.969369	70800.626787	33.795636
866.912291	70918.237833	33.800653
867.906477	71039.121622	33.805671
868.688586	71154.555192	33.810688
869.566416	71279.815098	33.815706
870.431977	71408.547788	33.820724
871.126070	71530.164744	33.825741
871.927341	71658.047481	33.830759
872.570759	71788.134001	33.835776
873.730563	71904.258971	33.840794
874.677351	72030.993503	33.845812
875.562551	72157.054345	33.850829
876.506487	72286.070348	33.855847
877.324379	72413.016876	33.860864
878.385950	72531.705784	33.865882
878.821765	72660.309205	33.870900
879.977965	72774.690674	33.875917
880.863054	72906.619390	33.880935
881.416828	73041.450484	33.885952
882.560639	73156.988142	33.890970
883.327705	73288.443253	33.895988
884.410745	73419.748207	33.901005
885.307210	73548.752434	33.906023
886.516093	73675.694425	33.911040
887.285479	73786.201587	33.916058
888.119369	73922.969219	33.921076
888.956430	74025.448937	33.926093
890.138545	74137.590228	33.931111
890.690171	74261.293950	33.936128
891.349078	74366.564178	33.941146
892.547706	74476.246975	33.946164
893.231100	74590.621582	33.951181
894.129051	74705.558417	33.956199
895.181057	74815.620226	33.961216
896.313120	74925.581281	33.966234
897.502950	75043.032564	33.971252
898.561163	75169.536532	33.976269
899.377991	75269.566760	33.981287
900.021937	75383.748234	33.986304
901.305882	75478.183241	33.991322
902.154839	75596.564337	33.996340
902.827804	75709.931942	34.001357
903.605148	75825.741133	34.006375
904.450848	75937.752577	34.011392
905.284477	76066.601358	34.016410
905.470028	76190.041876	34.021428
906.574360	76312.579039	34.026445
907.233151	76438.416751	34.031463
908.261758	76580.373723	34.036480
909.477669	76698.727495	34.041498
910.343969	76828.524842	34.046516
910.990704	76961.296120	34.051533
912.045787	77084.756547	34.056551
912.715755	77221.832532	34.061568
913.972982	77346.225251	34.066586
914.723205	77491.853592	34.071604
915.712929	77611.868244	34.076621
916.874693	77756.458105	34.081639
917.599875	77893.693485	34.086656
918.013464	78017.055857	34.091674
919.238174	78164.830423	34.096692
920.024854	78299.106460	34.101709
921.111994	78438.998926	34.106727
921.943242	78587.394775	34.111744
922.619029	78721.943601	34.116762
923.599985	78855.710514	34.121780
924.506334	79012.660923	34.126797
925.654908	79150.621714	34.131815
926.617867	79295.896870	34.136832
927.648310	79432.255937	34.141850
928.939872	79572.502185	34.146868
929.772600	79716.292313	34.151885
930.629838	79844.622980	34.156903
931.814552	79989.537635	34.161920
932.916332	80107.607169	34.166938
933.453919	80247.620127	34.171956
934.318765	80388.735458	34.176973
936.328786	80516.115878	34.181991
937.346222	80643.322886	34.187008
938.002334	80762.706576	34.192026
939.227942	80895.190678	34.197044
940.373783	81022.886085	34.202061
941.557075	81141.517348	34.207079
942.327871	81266.459903	34.212096
943.232706	81380.169214	34.217114
944.196684	81505.526026	34.222132
944.819335	81624.766571	34.227149
945.549738	81740.177077	34.232167
946.505091	81876.357069	34.237184
947.475735	82003.906968	34.242202
948.467965	82123.142428	34.247220
949.072672	82254.209708	34.252237
950.080990	82380.868488	34.257255
950.495451	82519.429580	34.262272
951.836453	82640.715884	34.267290
953.240448	82762.094205	34.272308
954.146374	82883.627052	34.277325
955.359003	82992.378481	34.282343
955.932302	83105.855198	34.287360
956.638253	83223.366209	34.292378
957.835043	83338.874902	34.297396
958.362805	83468.147902	34.302413
959.602742	83584.727848	34.307431
960.500439	83718.911020	34.312448
961.256014	83848.213419	34.317466
962.146556	83971.767979	34.322484
963.157179	84106.011306	34.327501
964.493740	84226.899563	34.332519
964.783265	84361.548422	34.337536
965.621409	84484.948665	34.342554
966.543854	84625.201706	34.347572
967.474093	84765.365508	34.352589
968.268644	84916.169874	34.357607
969.616853	85056.003544	34.362624
970.598185	85171.033801	34.367642
971.836769	85310.277632	34.372660
973.225144	85439.107934	34.377677
974.202428	85579.914568	34.382695
975.195897	85712.026524	34.387712
976.384587	85841.827588	34.392730
977.022023	85975.618477	34.397748
978.170458	86105.921225	34.402765
979.599850	86233.278681	34.407783
980.155547	86375.663135	34.412800
980.794489	86500.877224	34.417818
981.551732	86643.370817	34.422836
982.258505	86790.422333	34.427853
983.582843	86928.291867	34.432871
984.342438	87071.268718	34.437888
985.420542	87223.561304	34.442906
986.412533	87373.384357	34.447924
987.056462	87520.943594	34.452941
988.070546	87665.759022	34.457959
989.179113	87825.590149	34.462976
990.130533	87954.613993	34.467994
991.752356	88107.396288	34.473012
992.484788	88261.737982	34.478029
993.388067	88401.441857	34.483047
994.330657	88554.193400	34.488064
995.215721	88708.830346	34.493082
996.221872	88847.658446	34.498100
997.161300	89008.485586	34.503117
998.745724	89157.870060	34.508135
999.525874	89299.460395	34.513152
1000.681556	89445.250853	34.518170
1001.798708	89597.967742	34.523188
1002.562704	89742.629673	34.528205
1004.412548	89866.071544	34.533223
1005.777064	90006.534502	34.538240
1006.782788	90129.121078	34.543258
1008.000856	90265.996191	34.548276
1008.596265	90408.330416	34.553293
1009.782085	90534.413754	34.558311
1010.431745	90673.268111	34.563328
1011.827516	90802.957103	34.568346
1012.705321	90935.706136	34.573364
1013.366311	91070.428825	34.578381
1014.602502	91212.032811	34.583399
1015.574785	91341.346824	34.588416
1016.481933	91481.723498	34.593434
1017.956804	91623.304711	34.598452
1018.450670	91760.921019	34.603469
1019.365664	91887.356578	34.608487
1020.339216	92019.778504	34.613504
1021.416658	92141.550841	34.618522
1022.466157	92265.850274	34.623540
1023.363356	92397.791487	34.628557
1024.134970	92536.014209	34.633575
1025.074149	92660.624036	34.638592
1026.000759	92806.504583	34.643610
1027.023721	92946.058677	34.648628
1027.811289	93084.256024	34.653645
1028.728591	93227.262830	34.658663
1029.569385	93382.120727	34.663680
1030.510074	93533.465445	34.668698
1031.521637	93677.790467	34.673716
1032.145419	93836.715311	34.678733
1033.222031	93984.821463	34.683751
1034.153622	94147.945922	34.688768
1034.817153	94316.918533	34.693786
1035.896628	94466.648989	34.698804
1036.875110	94636.309203	34.703821
1038.122976	94806.967564	34.708839
1039.677606	94971.025521	34.713856
1040.365233	95128.007602	34.718874
1041.600722	95286.882118	34.723892
1042.461307	95460.824338	34.728909
1043.917461	95628.640543	34.733927
1044.732967	95796.773441	34.738944
1045.985508	95954.748681	34.743962
1047.091080	96112.253356	34.748980
1048.544543	96277.348088	34.753997
1049.746598	96442.939391	34.759015
1050.446908	96594.007013	34.764032
1051.320418	96753.807609	34.769050
1052.769710	96919.134527	34.774068
1053.373791	97087.053877	34.779085
1054.524458	97262.938164	34.784103
1055.524007	97427.691641	34.789120
1056.175521	97598.052858	34.794138
1057.719170	97761.569299	34.799156
1058.885431	97946.785029	34.804173
1059.709974	98113.344209	34.809191
1060.748689	98288.934765	34.814208
1061.929193	98456.897857	34.819226
1063.058445	98630.092824	34.824244
1064.158924	98798.856216	34.829261
1065.216227	98974.346197	34.834279
1066.302247	99140.628906	34.839296
1067.417471	99320.840345	34.844314
1068.607222	99490.632932	34.849332
1069.609276	99656.132764	34.854349
1070.630426	99820.476792	34.859367
1071.809073	99999.173449	34.864384
1072.798324	100164.056675	34.869402
1074.479513	100330.455162	34.874420
1075.331337	100507.177336	34.879437
1076.682712	100670.256890	34.884455
1078.237998	100828.500383	34.889472
1079.221920	100982.586955	34.894490
1080.213070	101138.156457	34.899508
1081.373592	101307.164384	34.904525
1082.836836	101460.138551	34.909543
1083.640543	101618.224608	34.914560
1084.751314	101772.256996	34.919578
1085.989695	101931.988085	34.924596
1086.893105	102090.897576	34.929613
1087.496361	102256.840690	34.934631
1088.522251	102416.645426	34.939648
1089.135237	102585.099023	34.944666
1090.287322	102753.443717	34.949684
1091.439565	102905.560408	34.954701
1092.523122	103059.007148	34.959719
1093.590730	103221.116775	34.964736
1094.403894	103386.652307	34.969754
1095.448560	103544.291426	34.974772
1096.111505	103712.337176	34.979789
1096.932095	103888.879475	34.984807
1098.465904	104055.548051	34.989824
1099.343350	104243.266377	34.994842
1100.401605	104415.120941	34.999860
1101.523180	104594.688229	35.004877
1102.928918	104755.788710	35.009895
1104.086046	104934.895783	35.014912
1105.029509	105122.824225	35.019930
1106.078413	105282.017740	35.024948
1107.454160	105466.139907	35.029965
1108.177094	105641.324575	35.034983
1109.456567	105815.218428	35.040000
1110.255514	106010.630170	35.045018
1111.579600	106189.628966	35.050036
1112.804217	106373.386620	35.055053
1114.144862	106553.323054	35.060071
1115.197534	106734.370654	35.065088
1116.274056	106923.708377	35.070106
1117.410069	107103.020356	35.075124
1118.504578	107291.292137	35.080141
1120.005892	107475.950724	35.085159
1121.570057	107646.892789	35.090176
1122.719552	107829.883793	35.095194
1123.674361	108000.060719	35.100212
1125.149589	108177.549875	35.105229
1126.301666	108348.534556	35.110247
1127.131838	108522.994305	35.115264
1128.304213	108713.696349	35.120282
1129.055029	108891.860518	35.125300
1129.998104	109068.778114	35.130317
1130.720767	109269.673082	35.135335
1132.228103	109450.245201	35.140352
1133.484870	109643.196348	35.145370
1134.816567	109834.019040	35.150388
1136.182416	110027.183479	35.155405
1136.872689	110204.628261	35.160423
1138.125740	110394.312280	35.165440
1139.017586	110588.086614	35.170458
1140.537298	110773.761575	35.175476
1141.685729	110969.463481	35.180493
1142.963436	111163.307361	35.185511
1144.224809	111347.630761	35.190528
1145.298645	111539.251226	35.195546
1146.580158	111710.891403	35.200564
1148.073909	111910.716787	35.205581
1148.898048	112092.715561	35.210599
1150.210563	112278.202499	35.215616
1150.915141	112464.622596	35.220634
1152.374617	112657.266645	35.225652
1153.456095	112838.011389	35.230669
1154.363772	113034.738791	35.235687
1156.170928	113212.581656	35.240704
1156.910736	113405.684779	35.245722
1158.023749	113593.619386	35.250740
1159.192212	113783.943317	35.255757
1160.189559	113962.474663	35.260775
1161.447523	114151.708462	35.265792
1162.523780	114348.175588	35.270810
1163.667237	114527.840962	35.275828
1164.865045	114717.695881	35.280845
1165.930521	114902.600714	35.285863
1167.183450	115090.356210	35.290880
1168.669596	115282.046007	35.295898
1169.712633	115452.866020	35.300916
1170.544105	115630.315291	35.305933
1171.325953	115808.381983	35.310951
1172.950634	115981.941780	35.315968
1174.021832	116167.131062	35.320986
1175.336338	116347.285831	35.326004
1176.567408	116528.494592	35.331021
1177.239705	116717.668305	35.336039
1178.350252	116909.070133	35.341056
1179.351029	117104.650428	35.346074
1180.529519	117297.172460	35.351092
1181.813766	117494.435417	35.356109
1182.550209	117699.661967	35.361127
1184.033434	117884.097587	35.366144
1185.032825	118086.393087	35.371162
1186.717016	118282.899910	35.376180
1188.255912	118475.815461	35.381197
1189.476990	118673.741341	35.386215
1190.731607	118864.052321	35.391232
1191.364476	119060.258406	35.396250
1192.730465	119260.904494	35.401268
1193.892504	119461.520134	35.406285
1195.437521	119666.009130	35.411303
1196.558313	119857.398814	35.416320
1198.215800	120055.834314	35.421338
1199.099927	120244.561092	35.426356
1200.416410	120441.377542	35.431373
1201.856496	120635.270767	35.436391
1203.429221	120828.852437	35.441408
1204.221896	121027.783470	35.446426
1205.695028	121220.697676	35.451444
1206.781299	121413.191354	35.456461
1208.406063	121597.990469	35.461479
1209.853061	121788.526717	35.466496
1211.169871	121977.092649	35.471514
1212.040951	122164.042084	35.476532
1213.545120	122348.432293	35.481549
1214.987089	122548.246166	35.486567
1215.910867	122735.824336	35.491584
1216.860867	122925.682726	35.496602
1218.068399	123114.474153	35.501620
1219.510371	123292.814657	35.506637
1220.431977	123493.831097	35.511655
1222.038447	123685.302939	35.516672
1222.969013	123896.862080	35.521690
1223.757146	124084.810342	35.526708
1225.323390	124284.841800	35.531725
1226.153231	124490.647606	35.536743
1227.624785	124684.923618	35.541760
1228.830896	124886.181573	35.546778
1230.333891	125075.785945	35.551796
1231.884202	125275.913601	35.556813
1232.586860	125471.595081	35.561831
1233.743165	125672.141586	35.566848
1234.806968	125867.692308	35.571866
1235.757773	126081.999998	35.576884
1237.093006	126285.807367	35.581901
1238.179504	126500.210177	35.586919
1239.744798	126699.809594	35.591936
1240.794046	126909.462753	35.596954
1241.721755	127128.232638	35.601972
1243.224031	127326.385925	35.606989
1244.253192	127544.799569	35.612007
1245.438250	127747.889097	35.617024
1246.275538	127963.987824	35.622042
1247.806252	128190.230541	35.627060
1249.432074	128396.489507	35.632077
1250.423663	128591.874054	35.637095
1252.486403	128780.139031	35.642112
1253.789453	128973.154761	35.647130
1254.741268	129163.244744	35.652148
1256.115538	129342.269165	35.657165
1257.046378	129549.340379	35.662183
1258.462370	129744.930254	35.667200
1259.733687	129945.479281	35.672218
1260.251834	130151.882122	35.677236
1261.807279	130350.447306	35.682253
1262.554924	130567.156984	35.687271
1263.882288	130780.211625	35.692288
1264.655775	130994.813171	35.697306
1265.852589	131216.036251	35.702324
1267.599846	131432.720677	35.707341
1268.307776	131647.462600	35.712359
1269.684206	131884.864103	35.717376
1271.202634	132105.051659	35.722394
1272.468512	132327.436925	35.727412
1273.955971	132555.308215	35.732429
1274.861161	132788.880268	35.737447
1276.310101	133008.499550	35.742464
1277.771123	133235.439524	35.747482
1278.943415	133469.252517	35.752500
1280.497239	133684.747513	35.757517
1281.422922	133916.190547	35.762535
1283.104038	134152.110001	35.767552
1284.745268	134376.032943	35.772570
1285.901688	134612.811001	35.777588
1287.795141	134828.842054	35.782605
1289.073925	135048.066578	35.787623
1290.228002	135268.466427	35.792640
1291.760513	135484.112986	35.797658
1293.084572	135711.112313	35.802676
1294.697828	135933.841848	35.807693
1295.801744	136151.195624	35.812711
1297.395518	136361.646655	35.817728
1298.373001	136590.100477	35.822746
1299.331809	136816.692943	35.827764
1300.510129	137034.432640	35.832781
1301.678083	137269.040021	35.837799
1302.606907	137490.551785	35.842816
1303.928934	137728.246441	35.847834
1305.525055	137961.737015	35.852852
1306.905703	138197.749780	35.857869
1307.949907	138437.699644	35.862887
1309.229128	138668.844877	35.867904
1310.263690	138909.141296	35.872922
1311.542351	139162.560810	35.877940
1313.056810	139404.332870	35.882957
1314.032149	139648.893664	35.887975
1315.540295	139880.491222	35.892992
1316.743134	140131.744965	35.898010
1318.241424	140376.202242	35.903028
1319.578811	140622.208860	35.908045
1320.963034	140865.950408	35.913063
1322.822040	141100.747824	35.918080
1324.097758	141341.272535	35.923098
1325.302722	141585.375731	35.928116
1327.223864	141809.366660	35.933133
1328.059784	142044.963343	35.938151
1329.666981	142284.323982	35.943168
1331.080710	142516.202754	35.948186
1331.865511	142759.235340	35.953204
1333.390902	142998.891468	35.958221
1334.269034	143242.812917	35.963239
1335.256336	143486.540790	35.968256
1336.766481	143727.865427	35.973274
1337.918880	143970.795625	35.978292
1339.427170	144197.768409	35.983309
1340.632754	144431.364006	35.988327
1341.928352	144668.601879	35.993344
1343.249546	144912.868237	35.998362
1344.589363	145150.088750	36.003380
1345.989530	145392.948924	36.008397
1346.833610	145636.988828	36.013415
1348.310133	145883.672426	36.018432
1349.716597	146132.107024	36.023450
1351.145675	146381.034282	36.028468
1352.415628	146620.569852	36.033485
1353.753652	146875.314187	36.038503
1354.944058	147126.528955	36.043520
1356.873773	147377.553054	36.048538
1357.541324	147628.547454	36.053556
1359.466178	147877.708882	36.058573
1360.582515	148139.170451	36.063591
1362.341655	148391.279590	36.068608
1363.562028	148642.179581	36.073626
1364.615531	148902.169671	36.078644
1366.105521	149157.573975	36.083661
1367.643750	149410.953741	36.088679
1369.639087	149654.324397	36.093696
1371.410012	149908.050874	36.098714
1372.461962	150152.269567	36.103732
1374.380089	150402.268877	36.108749
1375.636564	150647.536714	36.113767
1377.260846	150899.297905	36.118784
1378.466175	151134.357693	36.123802
1379.717735	151388.223122	36.128820
1381.501307	151639.277313	36.133837
1382.871196	151885.929215	36.138855
1383.799935	152140.407142	36.143872
1385.466174	152383.435226	36.148890
1386.434091	152646.261845	36.153908
1387.755446	152888.724102	36.158925
1389.169556	153160.876781	36.163943
1390.479116	153415.326259	36.168960
1392.135868	153663.654759	36.173978
1393.384473	153925.351691	36.178996
1394.857497	154178.090668	36.184013
1396.605251	154418.715517	36.189031
1398.170145	154666.732694	36.194048
1400.126560	154913.153635	36.199066
1401.226162	155171.096630	36.204084
1402.889425	155411.345304	36.209101
1404.219828	155668.733900	36.214119
1405.387457	155917.897625	36.219136
1407.054346	156159.595981	36.224154
1408.017673	156419.774665	36.229172
1409.333292	156674.034376	36.234189
1410.798044	156928.056019	36.239207
1412.053572	157183.939550	36.244224
1413.437083	157432.720383	36.249242
1414.834075	157703.729010	36.254260
1415.950733	157961.389488	36.259277
1417.184651	158226.065775	36.264295
1418.502964	158489.739783	36.269312
1419.437990	158756.191690	36.274330
1420.837165	159028.538866	36.279348
1422.454571	159305.232963	36.284365
1423.465984	159581.985063	36.289383
1424.911782	159850.431085	36.294400
1426.182301	160138.647140	36.299418
1427.491508	160417.222565	36.304436
1429.027610	160700.943503	36.309453
1431.027854	160980.720899	36.314471
1432.202812	161240.607603	36.319488
1433.582089	161514.136697	36.324506
1434.795618	161778.437669	36.329524
1436.172199	162037.991352	36.334541
1437.308727	162304.071254	36.339559
1438.746040	162585.403787	36.344576
1440.478532	162864.748844	36.349594
1442.146043	163140.804291	36.354612
1443.844389	163413.021845	36.359629
1445.835055	163657.936114	36.364647
1447.654998	163927.724487	36.369664
1449.432622	164187.719065	36.374682
1450.790145	164438.169305	36.379700
1452.146971	164693.483292	36.384717
1453.519603	164950.852589	36.389735
1455.018387	165209.587033	36.394752
1456.431719	165473.173203	36.399770
1457.624533	165737.810629	36.404788
1458.891604	165998.031734	36.409805
1460.433140	166280.925163	36.414823
1461.489811	166564.682835	36.419840
1462.722702	166837.240940	36.424858
1464.210342	167121.009601	36.429876
1465.563066	167401.994520	36.434893
1466.775562	167690.811102	36.439911
1468.391350	167983.666854	36.444928
1469.747403	168268.412983	36.449946
1470.706168	168564.751354	36.454964
1472.001801	168877.188945	36.459981
1473.545427	169183.316668	36.464999
1474.965546	169482.379959	36.470016
1476.454714	169787.033162	36.475034
1477.632657	170103.265508	36.480052
1479.009437	170413.576498	36.485069
1480.461327	170725.121374	36.490087
1482.089929	171048.258087	36.495104
1483.798096	171371.498010	36.500122
1484.857567	171701.722940	36.505140
1486.179078	172013.103067	36.510157
1487.976632	172334.974436	36.515175
1489.553911	172659.941783	36.520192
1491.293607	172967.730334	36.525210
1493.251321	173287.802894	36.530228
1494.841983	173595.160114	36.535245
1497.003842	173911.736729	36.540263
1498.459327	174227.180758	36.545280
1500.286720	174524.142944	36.550298
1501.414068	174839.209002	36.555316
1503.032836	175149.183600	36.560333
1504.611071	175451.800766	36.565351
1505.954612	175769.477806	36.570368
1507.705972	176071.955873	36.575386
1508.776432	176380.078087	36.580404
1510.419794	176693.216522	36.585421
1511.873663	177002.627044	36.590439
1513.181846	177325.979033	36.595456
1515.102085	177624.398134	36.600474
1516.992780	177936.638943	36.605492
1518.659482	178246.401612	36.610509
1519.976146	178556.347158	36.615527
1521.723010	178851.267394	36.620544
1523.244220	179151.328833	36.625562
1524.870288	179454.016225	36.630580
1526.469930	179756.505598	36.635597
1527.827107	180058.043427	36.640615
1529.408433	180361.832985	36.645632
1530.312349	180666.288333	36.650650
1532.353062	180979.608463	36.655668
1533.152451	181273.059444	36.660685
1534.892729	181559.404993	36.665703
1536.437433	181860.182836	36.670720
1537.954023	182149.028824	36.675738
1539.756814	182436.891159	36.680756
1541.216688	182730.471894	36.685773
1542.748209	183017.159303	36.690791
1544.315066	183324.262534	36.695808
1545.876344	183612.775746	36.700826
1546.966041	183916.145709	36.705844
1548.446385	184216.382199	36.710861
1550.273701	184517.555849	36.715879
1551.297566	184821.446851	36.720896
1552.833952	185139.583644	36.725914
1554.067208	185449.844329	36.730932
1555.819271	185764.825212	36.735949
1557.011160	186083.628428	36.740967
1558.835017	186402.689302	36.745984
1560.280819	186734.662453	36.751002
1562.196294	187055.285727	36.756020
1563.444416	187381.703928	36.761037
1565.227060	187719.875729	36.766055
1567.008368	188035.722367	36.771072
1568.410649	188380.204089	36.776090
1569.963397	188756.997477	36.781108
1571.439572	189078.482831	36.786125
1573.411129	189413.226626	36.791143
1574.895087	189752.441947	36.796160
1576.406689	190073.949963	36.801178
1578.402171	190396.780155	36.806196
1579.905726	190727.105142	36.811213
1581.819198	191055.614263	36.816231
1583.412358	191388.949719	36.821248
1584.745091	191720.853618	36.826266
1585.899337	192050.601896	36.831284
1587.656365	192394.277929	36.836301
1589.564893	192715.146673	36.841319
1591.007211	193064.969996	36.846336
1592.559341	193383.406929	36.851354
1594.095622	193724.936649	36.856372
1595.680231	194068.263180	36.861389
1597.903434	194395.411746	36.866407
1599.655895	194727.740435	36.871424
1601.370496	195050.779011	36.876442
1603.443713	195377.140610	36.881460
1604.902960	195700.677916	36.886477
1606.586435	196035.128908	36.891495
1607.912422	196366.639270	36.896512
1609.336290	196687.187016	36.901530
1611.383198	197008.069799	36.906548
1612.526660	197356.299881	36.911565
1614.398191	197689.531427	36.916583
1615.871256	198016.704250	36.921600
1617.127671	198361.007136	36.926618
1618.630144	198692.876162	36.931636
1620.118114	199038.236614	36.936653
1621.862856	199377.816790	36.941671
1623.299750	199720.900555	36.946688
1624.917348	200065.709520	36.951706
1626.737180	200413.662841	36.956724
1627.651219	200768.464842	36.961741
1629.433297	201109.084284	36.966759
1631.042352	201468.503816	36.971776
1632.332963	201827.973935	36.976794
1633.903068	202185.470467	36.981812
1635.634420	202535.270932	36.986829
1637.185312	202895.845593	36.991847
1638.542610	203255.892404	36.996864
1640.069551	203604.405967	37.001882
1642.160627	203945.185678	37.006900
1643.377010	204293.952326	37.011917
1645.028629	204634.573400	37.016935
1646.650161	204985.310089	37.021952
1648.280306	205338.281491	37.026970
1649.878841	205685.847627	37.031988
1651.294145	206055.746803	37.037005
1652.582445	206409.789627	37.042023
1654.155679	206777.810910	37.047040
1655.489067	207152.271914	37.052058
1657.375416	207525.884908	37.057076
1658.900782	207901.206204	37.062093
1660.505600	208278.725740	37.067111
1662.042349	208664.156927	37.072128
1663.620509	209049.277396	37.077146
1665.252338	209438.073532	37.082164
1666.630792	209822.337301	37.087181
1668.795971	210211.178133	37.092199
1670.445037	210604.037821	37.097216
1672.171491	210994.599639	37.102234
1675.210581	211363.668438	37.107252
1677.376803	211736.379985	37.112269
1679.265928	212104.486505	37.117287
1681.624834	212472.850188	37.122304
1683.242044	212840.695276	37.127322
1684.709390	213198.199540	37.132340
1686.590284	213560.466159	37.137357
1688.474730	213928.626253	37.142375
1689.969117	214303.833786	37.147392
1691.629168	214675.992724	37.152410
1693.109239	215041.880050	37.157428
1694.570026	215417.856031	37.162445
1696.253739	215791.587334	37.167463
1697.778418	216159.043694	37.172480
1699.406021	216542.691906	37.177498
1701.105128	216917.260057	37.182516
1702.873659	217298.143198	37.187533
1704.728451	217687.091564	37.192551
1705.965957	218069.252345	37.197568
1707.690299	218459.136205	37.202586
1709.548509	218834.442898	37.207604
1711.039704	219234.550718	37.212621
1713.095675	219614.831488	37.217639
1714.678612	220013.807617	37.222656
1715.850822	220409.647317	37.227674
1718.139903	220798.123081	37.232692
1719.119898	221212.995430	37.237709
1721.204465	221605.822207	37.242727
1722.498502	222021.179208	37.247744
1724.155782	222416.359481	37.252762
1725.830731	222827.643276	37.257780
1727.322924	223235.983491	37.262797
1729.799506	223637.259831	37.267815
1731.402435	224041.060934	37.272832
1733.422270	224444.415780	37.277850
1735.041334	224852.304493	37.282868
1736.718549	225254.519008	37.287885
1738.610089	225657.538317	37.292903
1740.442992	226057.340465	37.297920
1742.016835	226475.448654	37.302938
1744.096978	226881.563047	37.307956
1745.617940	227294.039683	37.312973
1747.175882	227698.685992	37.317991
1748.728108	228109.176030	37.323008
1750.354374	228524.125474	37.328026
1752.021549	228930.303982	37.333044
1753.934115	229341.296109	37.338061
1755.401536	229744.380862	37.343079
1757.181051	230135.095649	37.348096
1758.743525	230546.014991	37.353114
1760.697950	230945.161541	37.358132
1761.958288	231348.608137	37.363149
1763.787695	231752.879978	37.368167
1765.352010	232164.128316	37.373184
1766.590262	232582.438871	37.378202
1768.691902	232984.177680	37.383220
1770.117074	233410.663801	37.388237
1772.084766	233834.092409	37.393255
1773.686314	234260.473970	37.398272
1775.797986	234682.939328	37.403290
1777.954920	235112.154594	37.408308
1779.899325	235527.456009	37.413325
1781.518146	235954.442845	37.418343
1783.353372	236369.963672	37.423360
1785.034358	236804.484705	37.428378
1787.009353	237229.636058	37.433396
1789.069165	237658.914395	37.438413
1790.741514	238093.536744	37.443431
1792.664472	238514.858635	37.448448
1794.403593	238958.182742	37.453466
1796.514579	239381.658701	37.458484
1798.608536	239813.748463	37.463501
1800.424679	240235.821290	37.468519
1802.012342	240666.744174	37.473536
1803.527758	241107.356319	37.478554
1805.650505	241538.219434	37.483572
1807.764100	241971.877593	37.488589
1809.695489	242394.005049	37.493607
1811.356743	242823.566335	37.498624
1813.185108	243263.820773	37.503642
1815.145691	243702.885125	37.508660
1816.913674	244139.514654	37.513677
1818.517072	244577.312184	37.518695
1820.128076	245012.897566	37.523712
1821.737159	245469.211023	37.528730
1823.813758	245903.781741	37.533748
1825.576181	246350.847985	37.538765
1826.800207	246804.144881	37.543783
1829.048358	247262.259341	37.548800
1830.577561	247715.988924	37.553818
1832.245666	248176.782919	37.558836
1833.936441	248629.875251	37.563853
1835.646359	249091.828818	37.568871
1837.799113	249558.131833	37.573888
1839.984862	250026.790790	37.578906
1841.815342	250499.746154	37.583924
1843.546980	250954.299132	37.588941
1845.492920	251421.619858	37.593959
1847.446964	251878.827967	37.598976
1849.304394	252351.646533	37.603994
1850.661603	252820.782431	37.609012
1853.153810	253282.474373	37.614029
1855.058624	253741.487993	37.619047
1857.277996	254197.809167	37.624064
1859.314857	254658.247045	37.629082
1861.309011	255105.583002	37.634100
1863.197783	255564.872558	37.639117
1864.879643	256031.660856	37.644135
1866.873844	256486.383942	37.649152
1868.419949	256952.834598	37.654170
1870.265131	257403.056415	37.659188
1872.273290	257869.761634	37.664205
1873.649664	258344.615982	37.669223
1875.435166	258798.880817	37.674240
1877.055491	259259.291317	37.679258
1879.325036	259701.868994	37.684276
1881.007296	260146.137129	37.689293
1883.127508	260589.598442	37.694311
1885.096498	261026.426888	37.699328
1886.762796	261474.197621	37.704346
1888.743904	261921.028319	37.709364
1890.660993	262371.855006	37.714381
1892.722698	262813.233929	37.719399
1894.788757	263262.382650	37.724416
1896.255535	263709.438907	37.729434
1898.280789	264159.860207	37.734452
1899.979574	264618.153627	37.739469
1901.610858	265079.605075	37.744487
1903.551202	265539.990124	37.749504
1905.253870	266014.405068	37.754522
1907.322277	266466.079415	37.759540
1909.388137	266930.248247	37.764557
1911.004690	267410.968840	37.769575
1912.943271	267881.147108	37.774592
1915.010774	268353.842723	37.779610
1916.863651	268825.579030	37.784628
1918.872669	269299.015595	37.789645
1920.630146	269790.394624	37.794663
1922.508580	270263.465694	37.799680
1924.211507	270758.073555	37.804698
1925.632862	271253.256093	37.809716
1927.245297	271763.288814	37.814733
1929.287732	272263.549557	37.819751
1931.524980	272766.900770	37.824768
1932.850209	273286.239401	37.829786
1934.557761	273802.086475	37.834804
1936.396145	274326.163801	37.839821
1938.156602	274853.475362	37.844839
1940.183421	275371.827776	37.849856
1942.131733	275911.877439	37.854874
1943.854071	276442.892493	37.859892
1946.176019	276988.285767	37.864909
1948.139170	277521.719301	37.869927
1949.952465	278059.083527	37.874944
1951.810562	278610.252006	37.879962
1954.011289	279143.560979	37.884980
1956.043380	279691.545413	37.889997
1957.985186	280242.815877	37.895015
1960.567335	280790.680770	37.900032
1962.461974	281343.397878	37.905050
1964.520872	281882.524637	37.910068
1966.635411	282412.496845	37.915085
1968.932287	282959.348804	37.920103
1971.330994	283495.083630	37.925120
1973.512338	284019.649907	37.930138
1975.449284	284542.117434	37.935156
1977.633883	285071.093623	37.940173
1979.423813	285608.684814	37.945191
1981.409088	286125.038389	37.950208
1983.624770	286659.050401	37.955226
1985.738350	287181.901550	37.960244
1988.149161	287699.522086	37.965261
1990.261300	288223.634751	37.970279
1992.144012	288737.292366	37.975296
1994.764569	289257.381392	37.980314
1996.347961	289769.757199	37.985332
1998.916307	290284.513838	37.990349
2000.708446	290786.997028	37.995367
2003.293967	291283.105961	38.000384
2005.181726	291788.257467	38.005402
2007.361415	292283.253875	38.010420
2009.728775	292771.133112	38.015437
2011.355533	293266.284172	38.020455
2013.338029	293747.411272	38.025472
2014.584222	294231.061665	38.030490
2016.666231	294706.198939	38.035508
2018.589972	295185.546290	38.040525
2020.207485	295678.596705	38.045543
2022.031558	296155.742834	38.050560
2023.902776	296651.563356	38.055578
2026.041599	297152.186810	38.060596
2028.092119	297636.495322	38.065613
2029.372057	298141.154112	38.070631
2031.308475	298645.629476	38.075648
2033.378993	299156.705305	38.080666
2035.220871	299679.007770	38.085684
2037.557052	300192.799566	38.090701
2039.567406	300707.957576	38.095719
2042.019478	301216.390400	38.100736
2043.927515	301737.241060	38.105754
2045.785063	302260.455392	38.110772
2047.290358	302782.018845	38.115789
2049.470541	303312.153245	38.120807
2051.893315	303840.949679	38.125824
2053.839780	304381.669849	38.130842
2055.814200	304924.943785	38.135860
2058.368190	305453.728514	38.140877
2059.699637	305990.872595	38.145895
2061.826435	306540.679819	38.150912
2064.052944	307091.049227	38.155930
2066.096993	307646.340009	38.160948
2067.908292	308186.380604	38.165965
2070.293027	308751.961760	38.170983
2072.788703	309303.457325	38.176000
2074.636300	309860.632007	38.181018
2076.513768	310406.145458	38.186036
2078.911316	310955.860748	38.191053
2081.120301	311521.386116	38.196071
2082.700411	312087.003102	38.201088
2085.055542	312648.583450	38.206106
2086.925427	313217.288591	38.211124
2089.338885	313781.790197	38.216141
2091.286641	314353.260928	38.221159
2093.321947	314915.016021	38.226176
2095.052534	315491.988329	38.231194
2097.076560	316067.739949	38.236212
2099.310845	316641.141878	38.241229
2101.570552	317230.850351	38.246247
2103.463604	317811.599353	38.251264
2105.528231	318392.922899	38.256282
2107.251971	318971.297595	38.261300
2109.416972	319568.399472	38.266317
2111.580837	320160.037423	38.271335
2114.031303	320750.784981	38.276352
2116.117340	321344.093528	38.281370
2118.193433	321941.759825	38.286388
2120.255499	322524.245810	38.291405
2122.675872	323119.151776	38.296423
2125.103374	323712.855549	38.301440
2127.354835	324311.526179	38.306458
2129.357485	324892.719528	38.311476
2131.628125	325485.178961	38.316493
2133.909803	326071.208798	38.321511
2136.112135	326658.409661	38.326528
2138.476424	327243.851323	38.331546
2140.164316	327840.934173	38.336564
2142.636617	328425.199852	38.341581
2144.729211	329007.841825	38.346599
2146.912211	329595.890224	38.351616
2149.473016	330173.925689	38.356634
2151.392995	330755.604516	38.361652
2153.811695	331311.446958	38.366669
2155.690814	331860.643058	38.371687
2157.903327	332420.256223	38.376704
2160.217256	332977.130905	38.381722
2162.059650	333531.509023	38.386740
2164.439141	334087.266237	38.391757
2165.957023	334645.610568	38.396775
2168.061882	335206.036207	38.401792
2169.747650	335785.467368	38.406810
2171.951259	336370.185917	38.411828
2173.869412	336942.181070	38.416845
2176.009325	337527.093988	38.421863
2178.112606	338114.311359	38.426880
2180.369329	338704.741756	38.431898
2182.181666	339307.558658	38.436916
2184.577297	339901.752103	38.441933
2186.574878	340503.987131	38.446951
2188.571935	341109.052545	38.451968
2191.410193	341711.110045	38.456986
2194.036653	342292.546097	38.462004
2196.444741	342892.469394	38.467021
2198.950714	343494.167569	38.472039
2201.119572	344090.252651	38.477056
2203.263799	344696.677952	38.482074
2205.179235	345302.544983	38.487092
2207.723103	345910.128701	38.492109
2209.846967	346530.598467	38.497127
2211.679553	347147.273291	38.502144
2214.225581	347752.465012	38.507162
2216.300950	348359.215386	38.512180
2218.539808	348975.133422	38.517197
2220.815101	349597.931033	38.522215
2223.194725	350207.033866	38.527232
2226.037113	350826.220254	38.532250
2228.140158	351441.149485	38.537268
2230.183082	352058.561079	38.542285
2232.180671	352681.799188	38.547303
2234.430135	353311.577505	38.552320
2236.904846	353943.995459	38.557338
2238.786314	354567.468240	38.562356
2240.737172	355196.013454	38.567373
2242.600266	355841.595634	38.572391
2245.004481	356476.635385	38.577408
2247.679585	357108.831245	38.582426
2249.909797	357748.942053	38.587444
2252.904281	358369.781528	38.592461
2255.192803	358999.109125	38.597479
2257.394023	359631.555129	38.602496
2260.278466	360259.597328	38.607514
2262.274801	360890.401415	38.612532
2264.333796	361516.366629	38.617549
2267.019381	362142.930362	38.622567
2268.919067	362775.711996	38.627584
2271.189524	363403.479872	38.632602
2273.465011	364039.445046	38.637620
2276.173509	364664.659029	38.642637
2278.303245	365293.320751	38.647655
2280.583440	365930.460375	38.652672
2282.549751	366556.814051	38.657690
2284.541354	367201.953394	38.662708
2286.934211	367834.902539	38.667725
2288.810272	368481.602165	38.672743
2290.388471	369139.153650	38.677760
2293.038617	369789.756615	38.682778
2295.353446	370429.957530	38.687796
2297.778177	371084.391807	38.692813
2299.761399	371741.464163	38.697831
2301.821705	372396.938013	38.702848
2304.457439	373031.657395	38.707866
2306.026063	373668.809229	38.712884
2308.178230	374313.176720	38.717901
2310.614370	374950.365609	38.722919
2312.528065	375603.809466	38.727936
2314.821287	376240.964979	38.732954
2317.128409	376900.649099	38.737972
2319.693954	377549.687828	38.742989
2321.964911	378202.100547	38.748007
2324.356465	378843.054259	38.753024
2326.642511	379509.617522	38.758042
2328.784227	380180.619097	38.763060
2331.231980	380838.511345	38.768077
2333.606066	381505.997837	38.773095
2336.011928	382179.338145	38.778112
2338.400269	382853.119532	38.783130
2340.082983	383549.660453	38.788148
2342.652885	384221.883290	38.793165
2344.563010	384910.956552	38.798183
2347.018326	385604.458833	38.803200
2349.760319	386298.505009	38.808218
2351.819959	387004.236526	38.813236
2353.980382	387700.892508	38.818253
2356.537795	388414.989178	38.823271
2358.787686	389131.341622	38.828288
2360.913310	389842.299671	38.833306
2363.060094	390563.006999	38.838324
2365.144879	391290.741298	38.843341
2368.076248	392014.068149	38.848359
2370.430527	392751.691705	38.853376
2373.361367	393459.785508	38.858394
2375.719899	394182.985223	38.863412
2378.204947	394910.699932	38.868429
2380.917386	395632.787901	38.873447
2382.968592	396369.183188	38.878464
2385.619785	397101.209297	38.883482
2388.209702	397833.627236	38.888500
2390.520324	398559.434662	38.893517
2392.924089	399289.760721	38.898535
2395.320436	400021.988496	38.903552
2398.338892	400753.387194	38.908570
2401.120110	401472.956000	38.913588
2403.434531	402196.725550	38.918605
2405.828276	402924.053209	38.923623
2408.027171	403672.644222	38.928640
2410.566983	404390.640540	38.933658
2412.635492	405134.800705	38.938676
2415.233108	405869.997664	38.943693
2417.581475	406608.650499	38.948711
2419.808140	407345.375067	38.953728
2422.389966	408081.159464	38.958746
2424.295361	408835.341703	38.963764
2426.666487	409575.561899	38.968781
2429.797593	410328.185721	38.973799
2431.943832	411064.798547	38.978816
2434.960271	411791.992149	38.983834
2438.100292	412527.084577	38.988852
2440.935976	413271.710077	38.993869
2443.405378	413996.233858	38.998887
2445.686485	414730.575945	39.003904
2448.213778	415446.998610	39.008922
2450.866253	416170.711775	39.013940
2453.313383	416890.638888	39.018957
2455.888734	417606.576336	39.023975
2458.272797	418338.298924	39.028992
2460.954135	419040.161394	39.034010
2463.713704	419744.364899	39.039028
2466.163623	420450.413509	39.044045
2468.488144	421133.246556	39.049063
2470.601895	421804.004407	39.054080
2473.035850	422492.742185	39.059098
2475.307845	423181.937211	39.064116
2477.383865	423865.881158	39.069133
2479.616657	424561.608719	39.074151
2481.487384	425254.638862	39.079168
2484.148357	425960.666414	39.084186
2486.121806	426675.623870	39.089204
2488.084653	427396.219458	39.094221
2490.793895	428119.553742	39.099239
2492.632920	428845.019829	39.104256
2495.251128	429575.341734	39.109274
2497.889973	430319.988429	39.114292
2500.161903	431071.588855	39.119309
2502.759285	431826.445341	39.124327
2505.027630	432571.468826	39.129344
2507.670447	433323.227863	39.134362
2509.838495	434092.871247	39.139380
2512.290513	434854.202511	39.144397
2514.685142	435626.275961	39.149415
2517.007811	436424.352505	39.154432
2519.437231	437203.330020	39.159450
2521.851809	438004.256671	39.164468
2524.032728	438804.933412	39.169485
2526.765640	439600.084076	39.174503
2529.131003	440422.437987	39.179520
2531.821633	441235.510834	39.184538
2534.295102	442041.358604	39.189556
2536.547087	442873.775738	39.194573
2539.007266	443684.656001	39.199591
2541.442053	444529.041987	39.204608
2544.026565	445355.183684	39.209626
2546.803809	446195.954471	39.214644
2549.405335	447040.299554	39.219661
2552.409848	447872.725641	39.224679
2554.705208	448720.423778	39.229696
2557.574434	449564.154744	39.234714
2560.742157	450397.600044	39.239732
2563.188173	451251.416092	39.244749
2566.017410	452078.221754	39.249767
2569.060966	452912.124191	39.254784
2571.382866	453754.076350	39.259802
2574.385396	454594.720783	39.264820
2576.777959	455421.337156	39.269837
2579.852953	456250.028614	39.274855
2582.683799	457078.516936	39.279872
2585.168018	457911.259411	39.284890
2588.166571	458732.576565	39.289908
2591.182081	459555.668657	39.294925
2593.680421	460369.971149	39.299943
2596.410184	461196.258744	39.304960
2598.979127	462005.779344	39.309978
2601.631112	462829.830058	39.314996
2604.127378	463650.333272	39.320013
2607.156689	464463.750986	39.325031
2609.572022	465289.181589	39.330048
2612.044292	466105.835470	39.335066
2614.798141	466927.954106	39.340084
2616.791252	467737.843497	39.345101
2619.855161	468551.964411	39.350119
2622.419725	469378.782678	39.355136
2624.655565	470198.197106	39.360154
2627.170274	471028.520887	39.365172
2629.479173	471864.280909	39.370189
2632.325853	472684.483679	39.375207
2634.861839	473519.366694	39.380224
2637.386334	474340.846970	39.385242
2639.940671	475143.525220	39.390260
2642.338080	475958.892587	39.395277
2644.947764	476756.944015	39.400295
2647.647145	477567.544082	39.405312
2650.283812	478372.567774	39.410330
2652.522629	479185.929653	39.415348
2654.647033	480017.210861	39.420365
2656.953442	480837.029337	39.425383
2659.331395	481665.764503	39.430400
2662.012278	482500.808481	39.435418
2664.967229	483343.474801	39.440436
2667.540165	484204.446369	39.445453
2669.992695	485050.172230	39.450471
2673.775466	485888.942673	39.455488
2677.125904	486721.638875	39.460506
2680.240012	487548.684431	39.465524
2682.646205	488390.203245	39.470541
2685.402254	489225.878358	39.475559
2688.143288	490059.545367	39.480576
2691.030055	490904.022883	39.485594
2694.174502	491739.498329	39.490612
2696.600159	492582.442830	39.495629
2699.418013	493414.803978	39.500647
2702.176620	494264.148182	39.505664
2703.979145	495123.915727	39.510682
2706.604363	495984.008265	39.515700
2708.888645	496853.015457	39.520717
2711.872810	497715.317224	39.525735
2714.423378	498588.610459	39.530752
2716.803031	499471.190806	39.535770
2719.474352	500350.652037	39.540788
2722.195160	501248.473721	39.545805
2724.849303	502134.674601	39.550823
2727.228715	503048.442398	39.555840
2729.811181	503940.934738	39.560858
2732.931783	504835.098855	39.565876
2735.518704	505759.681305	39.570893
2738.162828	506658.535326	39.575911
2741.123155	507586.059990	39.580928
2743.903605	508511.237877	39.585946
2746.815777	509428.436897	39.590964
2749.127424	510363.727476	39.595981
2752.293022	511283.280523	39.600999
2755.071403	512207.762217	39.606016
2757.700693	513131.702872	39.611034
2760.403732	514060.247012	39.616052
2763.212539	515005.808314	39.621069
2766.029524	515944.666527	39.626087
2768.735393	516878.249181	39.631104
2771.642722	517818.171449	39.636122
2774.667248	518746.197360	39.641140
2777.467421	519692.139708	39.646157
2780.078054	520636.738780	39.651175
2782.999611	521579.011721	39.656192
2785.612863	522530.714750	39.661210
2788.542307	523476.521845	39.666228
2791.092557	524420.612834	39.671245
2793.913177	525367.056549	39.676263
2796.892925	526311.599199	39.681280
2799.944767	527266.713336	39.686298
2802.746182	528220.591811	39.691316
2805.439357	529187.728792	39.696333
2808.474587	530130.331036	39.701351
2810.735901	531069.018644	39.706368
2814.140941	532019.461928	39.711386
2816.382295	532964.343201	39.716404
2819.527159	533924.428974	39.721421
2822.376773	534866.866487	39.726439
2825.007393	535794.659713	39.731456
2828.349978	536698.529565	39.736474
2831.333619	537603.495830	39.741492
2834.203764	538509.620087	39.746509
2837.015297	539426.178394	39.751527
2840.009145	540324.072900	39.756544
2842.078138	541240.715931	39.761562
2844.785442	542158.296216	39.766580
2847.731247	543083.900346	39.771597
2849.948704	544010.603358	39.776615
2852.781375	544952.341956	39.781632
2855.233057	545900.038146	39.786650
2858.410773	546838.469277	39.791668
2860.744877	547805.951074	39.796685
2863.503411	548752.928655	39.801703
2866.488868	549720.709351	39.806720
2868.950321	550688.395033	39.811738
2872.181490	551669.070312	39.816756
2874.532948	552655.268750	39.821773
2877.067338	553644.215738	39.826791
2880.217819	554637.947959	39.831808
2883.006008	555641.879906	39.836826
2885.829830	556651.135074	39.841844
2889.033319	557659.143073	39.846861
2891.855736	558674.892501	39.851879
2894.796709	559685.726233	39.856896
2897.650191	560700.395251	39.861914
2901.064975	561717.444183	39.866932
2903.660340	562751.314575	39.871949
2906.563674	563778.734358	39.876967
2909.430297	564817.088118	39.881984
2911.974619	565855.950535	39.887002
2914.673741	566897.399820	39.892020
2917.686895	567949.872080	39.897037
2920.557172	569006.526234	39.902055
2923.414304	570070.444359	39.907072
2925.913833	571133.268352	39.912090
2928.858557	572200.428498	39.917108
2931.844721	573282.196105	39.922125
2934.912930	574359.093583	39.927143
2938.069676	575430.320341	39.932160
2941.197567	576525.465775	39.937178
2944.368526	577585.027366	39.942196
2946.919092	578682.953906	39.947213
2950.261186	579773.495904	39.952231
2953.504787	580844.640902	39.957248
2956.142499	581926.829098	39.962266
2959.699523	583007.017355	39.967284
2962.947225	584095.547841	39.972301
2965.758065	585186.588342	39.977319
2969.247105	586255.318650	39.982336
2972.094995	587335.090986	39.987354
2975.643297	588409.048799	39.992372
2978.235192	589486.198053	39.997389
2981.414536	590552.154692	40.002407
2984.716080	591623.432784	40.007424
2988.318993	592699.153055	40.012442
2991.903803	593747.742485	40.017460
2994.929917	594796.266177	40.022477
2998.475512	595846.153493	40.027495
3001.370564	596880.457238	40.032512
3004.492697	597935.596918	40.037530
3007.402181	598971.690739	40.042548
3010.474714	600015.794624	40.047565
3013.007658	601058.880343	40.052583
3016.256944	602082.831983	40.057600
3019.012658	603130.267749	40.062618
3021.931564	604149.775077	40.067636
3024.582297	605175.112100	40.072653
3027.468327	606190.979985	40.077671
3030.153102	607191.911636	40.082688
3032.798365	608204.973756	40.087706
3035.884371	609223.952043	40.092724
3038.569998	610236.507018	40.097741
3041.302573	611266.608024	40.102759
3044.543619	612300.314643	40.107776
3047.088697	613345.442391	40.112794
3050.015776	614396.584086	40.117812
3052.721544	615438.926700	40.122829
3055.646753	616493.139160	40.127847
3058.648206	617555.053248	40.132864
3061.448193	618638.065094	40.137882
3064.475066	619708.516054	40.142900
3067.480729	620806.705740	40.147917
3070.180119	621893.711837	40.152935
3073.825237	622993.102276	40.157952
3076.046707	624097.323728	40.162970
3079.403077	625211.502074	40.167988
3082.443325	626324.606654	40.173005
3085.132953	627452.525628	40.178023
3088.271177	628584.823309	40.183040
3091.383041	629728.192388	40.188058
3094.710094	630873.781159	40.193076
3097.470701	632027.234578	40.198093
3100.764782	633177.231260	40.203111
3104.276521	634328.896226	40.208128
3107.719412	635485.258063	40.213146
3111.080609	636634.577621	40.218164
3114.391489	637785.456355	40.223181
3117.592195	638940.985828	40.228199
3120.659086	640104.051522	40.233216
3123.642413	641264.649206	40.238234
3126.919663	642424.112222	40.243252
3130.453376	643591.244095	40.248269
3133.261214	644752.428600	40.253287
3136.951882	645905.328951	40.258304
3139.824239	647084.795124	40.263322
3143.282230	648249.859848	40.268340
3146.764022	649419.690463	40.273357
3149.417202	650596.553614	40.278375
3153.002049	651756.383597	40.283392
3155.817196	652922.889165	40.288410
3159.052719	654107.895966	40.293428
3162.584728	655274.581925	40.298445
3165.406186	656448.821901	40.303463
3168.695324	657611.420685	40.308480
3172.354423	658786.364900	40.313498
3175.483932	659959.451040	40.318516
3178.514129	661132.794893	40.323533
3181.715425	662311.413005	40.328551
3185.145729	663487.457642	40.333568
3187.979729	664667.009018	40.338586
3191.542757	665852.981726	40.343604
3194.580974	667033.521836	40.348621
3197.433491	668212.940108	40.353639
3200.811294	669395.387682	40.358656
3204.087414	670581.951915	40.363674
3207.351183	671769.841944	40.368692
3211.007679	672934.272117	40.373709
3214.325496	674115.340524	40.378727
3218.035784	675285.685096	40.383744
3220.809157	676466.613644	40.388762
3224.211753	677633.515384	40.393780
3227.394737	678801.776644	40.398797
3230.685891	679985.452877	40.403815
3234.062608	681139.204245	40.408832
3236.938563	682280.108364	40.413850
3240.206193	683411.939472	40.418868
3242.909777	684541.628124	40.423885
3245.600571	685692.634994	40.428903
3248.594857	686828.943713	40.433920
3251.528859	687981.426317	40.438938
3254.663442	689137.821510	40.443956
3257.838296	690306.112017	40.448973
3260.716375	691479.325560	40.453991
3264.263938	692652.316509	40.459008
3267.281892	693840.393927	40.464026
3270.402694	695024.082704	40.469044
3273.511380	696216.444867	40.474061
3276.010388	697414.111734	40.479079
3279.504380	698629.572041	40.484096
3282.829375	699852.184514	40.489114
3286.153606	701077.327233	40.494132
3289.299657	702314.899552	40.499149
3292.377807	703555.993278	40.504167
3295.785613	704798.175159	40.509184
3299.146436	706043.871441	40.514202
3302.143135	707303.637982	40.519220
3305.447773	708587.918560	40.524237
3309.087147	709862.320523	40.529255
3311.993926	711134.165063	40.534272
3314.997629	712410.028462	40.539290
3318.343028	713706.531766	40.544308
3321.565317	714995.002109	40.549325
3324.558883	716301.084537	40.554343
3328.376595	717607.360088	40.559360
3331.634919	718911.285486	40.564378
3335.150465	720231.499428	40.569396
3338.602566	721548.935625	40.574413
3341.688294	722872.603300	40.579431
3345.365084	724190.533970	40.584448
3348.630569	725527.004350	40.589466
3351.640690	726858.505793	40.594484
3355.294860	728190.754688	40.599501
3358.500094	729535.727228	40.604519
3362.465894	730872.421503	40.609536
3365.802608	732199.583056	40.614554
3369.134379	733557.681916	40.619572
3372.878188	734888.333287	40.624589
3375.789002	736248.562914	40.629607
3379.149620	737580.757046	40.634624
3382.851243	738953.535094	40.639642
3386.021744	740298.484111	40.644660
3389.624367	741640.368692	40.649677
3392.961550	743009.547137	40.654695
3396.266339	744365.217877	40.659712
3399.861303	745731.585764	40.664730
3403.336097	747097.027778	40.669748
3406.881253	748452.632607	40.674765
3410.373381	749809.854853	40.679783
3413.879718	751161.472061	40.684800
3417.649505	752521.522041	40.689818
3420.978257	753872.115102	40.694836
3424.785770	755217.180808	40.699853
3428.268471	756575.716634	40.704871
3431.873707	757922.946909	40.709888
3435.594234	759276.858871	40.714906
3438.670882	760626.790124	40.719924
3441.954022	761963.989796	40.724941
3445.489000	763327.678110	40.729959
3448.911013	764664.632543	40.734976
3452.237766	766023.125583	40.739994
3455.717757	767367.332627	40.745012
3459.161486	768694.608575	40.750016
3462.280330	769986.371191	40.755021
3465.664751	771228.717680	40.760026
3468.569848	772430.762274	40.765031
3471.709566	773571.875933	40.770036
3475.206084	774643.737999	40.775040
3477.787520	775654.272869	40.780045
3480.459334	776615.256252	40.785050
3483.902116	777501.226417	40.790055
3486.120536	778316.687995	40.795060
3488.960181	779058.537203	40.800064
3492.020004	779748.261813	40.805069
3494.286767	780380.698630	40.810074
3496.459147	780945.814938	40.815079
3498.361670	781485.075138	40.820084
3500.051403	781942.030059	40.825088
3502.298674	782357.501196	40.830093
3503.727595	782725.054033	40.835098
3505.137593	783055.291175	40.840103
3506.079769	783349.022504	40.845108
3507.796274	783590.837011	40.850112
3508.561108	783801.272457	40.855117
3509.668928	783980.569913	40.860122
3510.421354	784123.163976	40.865127
3511.277028	784253.357184	40.870132
3512.129228	784339.797259	40.875136
3512.891978	784401.438508	40.880141
3513.477800	784448.865904	40.885146
3513.981974	784468.998471	40.890151
3514.159549	784470.879313	40.895156
3515.054759	784445.095933	40.900160
3515.215095	784426.376550	40.905165
3515.703811	784372.516943	40.910170
3516.134642	784314.652957	40.915175
3516.510412	784237.514931	40.920180
3516.888534	784142.561428	40.925184
3517.132041	784037.937308	40.930189
3517.463918	783924.439270	40.935194
3517.776486	783791.854658	40.940199
3517.878187	783659.594039	40.945204
3518.336279	783511.368030	40.950208
3518.571953	783354.216389	40.955213
3518.323092	783188.668932	40.960218
3518.820586	783027.210265	40.965223
3518.524938	782845.949175	40.970228
3519.115331	782667.432775	40.975232
3519.201870	782477.192854	40.980237
3518.610394	782285.193267	40.985242
3518.654755	782087.507875	40.990247
3518.815147	781894.694180	40.995252
3519.026055	781684.780645	41.000256
3518.835010	781491.031110	41.005261
3518.557847	781265.807410	41.010266
3518.890928	781044.985340	41.015271
3518.822193	780836.557862	41.020276
3518.567809	780620.857008	41.025280
3518.844520	780413.978293	41.030285
3518.833410	780192.594399	41.035290
3518.695661	779960.449447	41.040295
3518.449868	779744.180437	41.045300
3518.476770	779513.218625	41.050304
3518.596407	779299.620754	41.055309
3518.154217	779081.842925	41.060314
3518.096873	778851.508300	41.065319
3517.490329	778641.578545	41.070324
3517.862451	778416.108932	41.075328
3517.322554	778196.162559	41.080333
3517.820427	777980.602414	41.085338
3517.885119	777745.753323	41.090343
3517.294598	777536.129591	41.095348
3517.223179	777298.101980	41.100352
3517.183848	777088.574170	41.105357
3516.924385	776871.676316	41.110362
3516.959381	776650.756905	41.115367
3516.730943	776439.131785	41.120372
3516.898509	776223.224335	41.125376
3516.351387	776015.114643	41.130381
3516.032113	775800.690827	41.135386
3516.601122	775593.226736	41.140391
3516.106893	775383.374314	41.145396
3516.256948	775165.769832	41.150400
3516.043146	774961.594188	41.155405
3515.610632	774754.212041	41.160410
3515.644468	774545.231359	41.165415
3515.553134	774346.164143	41.170420
3515.739606	774135.284584	41.175424
3515.590846	773940.037484	41.180429
3515.263012	773725.255467	41.185434
3514.943603	773517.229769	41.190439
3514.416009	773325.161387	41.195444
3514.823074	773129.461056	41.200448
3514.764681	772938.828080	41.205453
3514.638967	772742.954853	41.210458
3514.475868	772549.287950	41.215463
3514.082304	772362.809338	41.220468
3513.823791	772163.263328	41.225472
3513.826227	771988.233958	41.230477
3513.836755	771802.265233	41.235482
3513.503123	771614.825296	41.240487
3513.215939	771441.151050	41.245492
3513.312841	771254.663632	41.250496
3513.275695	771080.990205	41.255501
3513.059866	770908.860430	41.260506
3512.872451	770732.357571	41.265511
3512.975519	770553.647064	41.270516
3512.999298	770378.769411	41.275520
3512.475507	770220.205494	41.280525
3512.095884	770056.564036	41.285530
3512.950390	769877.816566	41.290535
3512.006111	769718.325927	41.295540
3512.127632	769563.030042	41.300544
3511.955317	769401.792875	41.305549
3511.910549	769237.245774	41.310554
3511.920405	769082.348885	41.315559
3511.388452	768927.876560	41.320564
3511.589134	768767.252928	41.325568
3511.320879	768619.550602	41.330573
3511.134887	768466.436368	41.335578
3511.219983	768313.178247	41.340583
3511.269514	768176.846472	41.345588
3511.119245	768020.479087	41.350592
3510.927315	767880.990528	41.355597
3510.807646	767735.110227	41.360602
3510.905075	767584.286932	41.365607
3510.639166	767441.514056	41.370612
3510.886665	767300.031703	41.375616
3510.196000	767150.892123	41.380621
3510.094294	767018.044581	41.385626
3510.376537	766874.389284	41.390631
3510.131370	766742.589240	41.395636
3510.276450	766612.737415	41.400640
3510.227244	766482.422852	41.405645
3509.736009	766341.821472	41.410650
3510.128403	766220.903187	41.415655
3509.468227	766086.849271	41.420660
3509.580259	765961.897452	41.425664
3509.743954	765835.904791	41.430669
3508.958353	765705.298150	41.435674
3509.629563	765582.754818	41.440679
3509.076163	765457.210895	41.445684
3509.022147	765343.512026	41.450688
3508.849142	765227.376073	41.455693
3508.732319	765109.904308	41.460698
3508.765044	764984.456518	41.465703
3508.595540	764882.301515	41.470708
3508.666217	764777.113606	41.475712
3508.659334	764660.942216	41.480717
3508.421881	764549.565811	41.485722
3508.414761	764437.366303	41.490727
3508.347425	764331.947827	41.495732
3508.573304	764210.971504	41.500736
3508.131687	764117.142928	41.505741
3507.859327	764008.266612	41.510746
3507.995255	763909.829129	41.515751
3507.599805	763807.595490	41.520756
3507.603071	763698.229461	41.525760
3507.491846	763594.917437	41.530765
3507.422892	763507.600175	41.535770
3507.090998	763419.881119	41.540775
3507.214443	763335.918785	41.545780
3507.374008	763246.157125	41.550784
3507.194393	763152.863683	41.555789
3506.964409	763055.404067	41.560794
3507.336187	762969.582110	41.565799
3506.988516	762881.073264	41.570804
3506.982783	762780.089143	41.575808
3506.812363	762693.759429	41.580813
3507.041287	762613.895844	41.585818
3506.659788	762530.100941	41.590823
3506.496921	762453.144301	41.595828
3506.697425	762365.426952	41.600832
3506.201318	762278.308372	41.605837
3506.255742	762200.382132	41.610842
3506.483081	762117.567257	41.615847
3506.050453	762049.486041	41.620852
3506.148493	761971.746831	41.625856
3506.078182	761899.384966	41.630861
3506.086501	761823.622131	41.635866
3506.008277	761746.104370	41.640871
3506.097362	761681.031372	41.645876
3505.666579	761613.633042	41.650880
3505.791062	761541.580739	41.655885
3505.598324	761465.796358	41.660890
3505.823605	761395.838226	41.665895
3505.774412	761325.824094	41.670900
3505.717656	761257.823725	41.675904
3505.871897	761197.941117	41.680909
3505.687285	761124.263277	41.685914
3505.923329	761045.019046	41.690919
3505.471655	760974.818794	41.695924
3505.520817	760910.039513	41.700928
3505.724814	760851.177410	41.705933
3505.395890	760783.755166	41.710938
3505.982305	760712.751612	41.715943
3505.169533	760655.765600	41.720948
3505.390442	760586.684034	41.725952
3505.230486	760525.764403	41.730957
3504.956565	760459.361741	41.735962
3505.360188	760400.759315	41.740967
3505.213720	760338.215303	41.745972
3504.925311	760274.563364	41.750976
3504.961519	760220.829776	41.755981
3504.986700	760162.922976	41.760986
3504.999729	760106.589198	41.765991
3504.462238	760058.542868	41.770996
3504.709376	759998.193486	41.776000
3504.594802	759956.661515	41.781005
3504.647347	759904.347244	41.786010
3504.607253	759850.229838	41.791015
3504.743031	759805.416297	41.796020
3504.895012	759755.295528	41.801024
3504.760071	759690.681120	41.806029
3504.642119	759636.672472	41.811034
3504.991672	759580.429217	41.816039
3504.568992	759530.052862	41.821044
3504.970894	759475.765247	41.826048
3504.493769	759425.003715	41.831053
3504.015639	759376.255793	41.836058
3504.242926	759326.758726	41.841063
3504.025574	759286.221218	41.846068
3503.932692	759239.769799	41.851072
3504.182479	759205.593325	41.856077
3504.311688	759150.314335	41.861082
3504.457359	759108.441956	41.866087
3504.254717	759069.079763	41.871092
3504.174633	759005.776719	41.876096
3504.503640	758967.018529	41.881101
3504.154820	758920.162925	41.886106
3504.172800	758869.663831	41.891111
3504.072690	758830.677245	41.896116
3504.238465	758794.055840	41.901120
3504.037396	758755.919690	41.906125
3503.813955	758714.446522	41.911130
3503.960321	758665.939907	41.916135
3503.865619	758624.003980	41.921140
3503.682960	758581.393829	41.926144
3503.740379	758552.549554	41.931149
3503.919687	758510.717488	41.936154
3503.718753	758466.193677	41.941159
3503.604415	758426.814088	41.946164
3503.763706	758394.416299	41.951168
3503.775808	758353.051556	41.956173
3503.589553	758323.753190	41.961178
3503.711911	758286.546438	41.966183
3503.848021	758243.687913	41.971188
3503.516567	758201.442602	41.976192
3503.586742	758171.563134	41.981197
3503.547389	758142.191923	41.986202
3503.629948	758108.527537	41.991207
3503.569221	758066.828615	41.996212
3503.536633	758030.922030	42.001216
3503.708293	757997.390566	42.006221
3503.313955	757961.147157	42.011226
3503.645632	757914.424121	42.016231
3503.516716	757889.339972	42.021236
3503.248593	757852.437611	42.026240
3502.959284	757825.560564	42.031245
3503.087515	757797.586444	42.036250
3503.535645	757758.360839	42.041255
3503.476114	757736.999092	42.046260
3503.533693	757706.087915	42.051264
3503.267219	757678.125894	42.056269
3503.028359	757645.639521	42.061274
3503.215859	757611.022894	42.066279
3502.954316	757587.186649	42.071284
3503.096119	757555.672087	42.076288
3502.892893	757521.853057	42.081293
3502.859213	757498.619588	42.086298
3503.048469	757479.723834	42.091303
3502.511994	757468.998943	42.096308
3503.164350	757440.057120	42.101312
3502.846669	757410.480717	42.106317
3502.863661	757393.429518	42.111322
3503.174373	757365.032109	42.116327
3502.891237	757350.287775	42.121332
3502.783660	757318.368953	42.126336
3502.793187	757294.391080	42.131341
3503.083246	757267.961793	42.136346
3503.022862	757243.061162	42.141351
3502.877007	757220.384771	42.146356
3502.883693	757188.103570	42.151360
3502.987685	757164.896616	42.156365
3502.791746	757147.976377	42.161370
3502.893215	757120.200292	42.166375
3502.955720	757094.297261	42.171380
3502.759714	757067.894076	42.176384
3503.105608	757036.443563	42.181389
3502.840321	757026.216075	42.186394
3502.556615	756996.878297	42.191399
3502.675464	756974.552811	42.196404
3502.553407	756952.363182	42.201408
3502.954298	756930.681350	42.206413
3502.843159	756905.885734	42.211418
3502.952386	756888.818900	42.216423
3502.887533	756868.487191	42.221428
3502.928633	756844.306317	42.226432
3503.020083	756819.085646	42.231437
3502.929440	756794.384706	42.236442
3503.013199	756763.563586	42.241447
3503.043305	756746.508777	42.246452
3502.660760	756717.283562	42.251456
3502.511677	756702.811734	42.256461
3502.504459	756672.987165	42.261466
3502.526407	756639.030435	42.266471
3502.419208	756634.330101	42.271476
3502.490848	756612.010851	42.276480
3502.562924	756594.064651	42.281485
3502.788210	756580.909886	42.286490
3502.509834	756554.026287	42.291495
3502.517404	756528.719420	42.296500
3502.394398	756511.049193	42.301504
3502.566101	756491.416483	42.306509
3502.286251	756484.089605	42.311514
3502.676495	756460.098527	42.316519
3502.657097	756449.389523	42.321524
3502.250677	756420.707329	42.326528
3502.282194	756420.063632	42.331533
3502.530141	756393.932496	42.336538
3502.442739	756375.863259	42.341543
3502.163671	756351.239365	42.346548
3502.451998	756350.997764	42.351552
3502.337828	756334.013654	42.356557
3502.131494	756313.407634	42.361562
3502.356613	756299.711845	42.366567
3502.308085	756286.943311	42.371572
3502.076257	756277.987122	42.376576
3501.870217	756277.773661	42.381581
3502.099499	756254.003605	42.386586
3502.292919	756241.639421	42.391591
3502.111073	756240.242831	42.396596
3501.812443	756213.655940	42.401600
3502.323394	756204.386986	42.406605
3502.015593	756197.015038	42.411610
3502.055532	756168.163764	42.416615
3502.440812	756170.707975	42.421620
3502.186291	756151.190092	42.426624
3502.540979	756131.871763	42.431629
3502.154955	756128.836303	42.436634
3502.248389	756104.890423	42.441639
3502.105553	756098.033128	42.446644
3502.375788	756089.391339	42.451648
3502.441302	756076.702879	42.456653
3502.189790	756061.656065	42.461658
3502.182607	756034.384113	42.466663
3502.166996	756023.968718	42.471668
3502.168197	756012.273014	42.476672
3502.347140	755992.146381	42.481677
3501.941065	755983.757610	42.486682
3502.052509	755977.990695	42.491687
3501.988757	755960.702960	42.496692
3502.390358	755946.340065	42.501696
3502.118324	755939.994227	42.506701
3501.877124	755918.311394	42.511706
3502.195135	755904.158048	42.516711
3502.134033	755894.683267	42.521716
3501.586144	755880.566949	42.526720
3501.758257	755869.728847	42.531725
3501.829321	755871.290306	42.536730
3502.140057	755863.821318	42.541735
3501.812559	755848.638503	42.546740
3501.835751	755847.160639	42.551744
3501.990627	755843.696505	42.556749
3501.824660	755830.650654	42.561754
3501.946745	755815.839768	42.566759
3501.478942	755811.146114	42.571764
3501.774626	755794.440636	42.576768
3501.828669	755803.818421	42.581773
3501.739340	755795.723907	42.586778
3501.910229	755769.848231	42.591783
3502.105471	755773.945717	42.596788
3502.314560	755773.077633	42.601792
3502.418089	755746.426120	42.606797
3502.289422	755741.826833	42.611802
3502.154108	755727.793144	42.616807
3502.057900	755712.475594	42.621812
3502.023754	755711.154095	42.626816
3502.209381	755694.269014	42.631821
3502.221628	755670.973222	42.636826
3502.407327	755658.314370	42.641831
3502.094981	755643.423606	42.646836
3502.400364	755633.547181	42.651840
3502.013371	755626.334447	42.656845
3501.983648	755603.929581	42.661850
3502.440758	755594.815685	42.666855
3502.136264	755586.951143	42.671860
3502.292744	755575.033869	42.676864
3502.236480	755564.624154	42.681869
3502.082872	755547.840900	42.686874
3501.843216	755536.182062	42.691879
3502.189282	755537.602318	42.696884
3501.874667	755524.628284	42.701888
3502.282774	755502.498666	42.706893
3502.002340	755499.839581	42.711898
3502.057826	755482.728619	42.716903
3502.088705	755466.751792	42.721908
3502.271209	755460.481901	42.726912
3502.275246	755445.737842	42.731917
3502.221849	755439.209941	42.736922
3502.172974	755423.638643	42.741927
3502.055442	755404.637882	42.746932
3501.789114	755390.378279	42.751936
3501.902078	755390.311500	42.756941
3501.931027	755388.685206	42.761946
3501.995812	755367.837470	42.766951
3502.288193	755359.486206	42.771956
3502.208412	755350.652509	42.776960
3502.304732	755335.795505	42.781965
3501.976491	755327.344638	42.786970
3502.110372	755305.552149	42.791975
3501.876684	755295.071482	42.796980
3501.937379	755284.151613	42.801985
3502.023457	755288.905344	42.806989
3501.968919	755274.170085	42.811994
3502.031338	755263.299061	42.816999
3501.538615	755255.119550	42.822004
3501.911589	755248.180798	42.827009
3502.101613	755226.870754	42.832013
3501.994181	755216.517673	42.837018
3502.104595	755208.440411	42.842023
3502.177380	755189.949936	42.847028
3502.095300	755183.966896	42.852033
3502.017665	755177.835717	42.857037
3502.047842	755173.751843	42.862042
3502.103221	755154.231914	42.867047
3501.961632	755150.125731	42.872052
3502.179972	755141.245169	42.877057
3502.290215	755116.900153	42.882061
3501.707169	755122.397509	42.887066
3502.179895	755104.778088	42.892071
3502.279988	755088.494706	42.897076
3501.911436	755088.110018	42.902081
3501.747885	755064.987161	42.907085
3501.961062	755058.564680	42.912090
3501.696717	755045.581909	42.917095
3501.708878	755057.424610	42.922100
3502.204311	755052.088395	42.927105
3502.137651	755025.755668	42.932109
3501.831815	755023.198668	42.937114
3501.818778	755012.879682	42.942119
3501.690994	754998.646780	42.947124
3501.986751	754986.166119	42.952129
3501.931378	754973.101400	42.957133
3501.687140	754976.727421	42.962138
3502.127337	754973.464003	42.967143
3501.626135	754957.765800	42.972148
3501.787596	754945.502655	42.977153
3501.892697	754944.552431	42.982157
3502.034979	754943.547247	42.987162
3502.170997	754921.851545	42.992167
3501.983176	754916.671186	42.997172
3502.308214	754909.444708	43.002177
3502.316442	754892.438009	43.007181
3501.903359	754886.703056	43.012186
3502.071176	754871.342417	43.017191
3501.932544	754856.078799	43.022196
3501.649711	754848.603240	43.027201
3502.006925	754837.341437	43.032205
3501.643742	754836.710149	43.037210
3501.711131	754815.024849	43.042215
3501.624329	754814.989294	43.047220
3501.771696	754808.183681	43.052225
3501.877172	754805.611454	43.057229
3501.634353	754811.645652	43.062234
3501.738444	754780.370393	43.067239
3501.405163	754778.505687	43.072244
3501.397811	754776.049385	43.077249
3501.886505	754780.691370	43.082253
3501.905876	754780.737516	43.087258
3501.926640	754783.240920	43.092263
3501.935243	754760.237606	43.097268
3501.625430	754756.894737	43.102273
3501.783850	754745.467266	43.107277
3501.782914	754750.284111	43.112282
3501.904951	754723.330968	43.117287
3501.905571	754719.792103	43.122292
3501.298231	754718.805771	43.127297
3501.582389	754712.912533	43.132301
3501.589443	754721.856744	43.137306
3501.390038	754712.746052	43.142311
3501.398110	754717.905560	43.147316
3501.443260	754707.478734	43.152321
3501.812164	754694.691229	43.157325
3501.713084	754692.986489	43.162330
3502.038314	754681.876892	43.167335
3501.816193	754686.728356	43.172340
3501.566433	754683.916715	43.177345
3501.896903	754661.452569	43.182349
3501.614021	754666.313545	43.187354
3501.310688	754659.627396	43.192359
3501.574237	754664.353803	43.197364
3501.563307	754655.066124	43.202369
3501.644941	754655.594042	43.207373
3501.252810	754642.925411	43.212378
3501.605916	754624.143891	43.217383
3501.711947	754617.836064	43.222388
3501.390939	754630.763722	43.227393
3501.582089	754632.552436	43.232397
3501.771151	754638.519267	43.237402
3501.833517	754636.494373	43.242407
3502.294870	754628.509045	43.247412
3502.219824	754607.582637	43.252417
3501.905933	754608.024936	43.257421
3501.854492	754587.094777	43.262426
3502.076036	754574.428394	43.267431
3502.098208	754568.870897	43.272436
3501.795585	754552.894998	43.277441
3501.671424	754534.040395	43.282445
3501.681292	754531.237259	43.287450
3501.870592	754529.733155	43.292455
3501.865267	754529.340803	43.297460
3501.543950	754516.660876	43.302465
3502.050361	754506.849769	43.307469
3501.766187	754500.307928	43.312474
3501.934683	754497.578284	43.317479
3501.629493	754500.722559	43.322484
3501.763491	754483.940979	43.327489
3501.627845	754481.062266	43.332493
3501.776392	754471.896873	43.337498
3501.761886	754475.880447	43.342503
3502.042180	754478.589145	43.347508
3501.591270	754459.343058	43.352513
3501.975307	754446.012073	43.357517
3501.888502	754442.486737	43.362522
3501.896728	754442.092262	43.367527
3501.929395	754415.545138	43.372532
3502.097115	754400.380107	43.377537
3501.836741	754397.815771	43.382541
3501.877075	754404.887396	43.387546
3502.006015	754385.108096	43.392551
3502.312474	754373.951801	43.397556
3502.177725	754375.398308	43.402561
3502.234442	754343.587859	43.407565
3501.905138	754342.508854	43.412570
3501.874215	754330.373029	43.417575
3502.138357	754305.067276	43.422580
3501.682537	754307.006362	43.427585
3501.965726	754292.560342	43.432589
3501.768573	754300.799711	43.437594
3501.835759	754272.526310	43.442599
3502.105582	754263.833221	43.447604
3501.743163	754257.303386	43.452609
3501.771902	754262.214228	43.457613
3501.561280	754252.809781	43.462618
3501.533361	754233.791878	43.467623
3501.734024	754224.421406	43.472628
3502.031496	754233.861518	43.477633
3502.234082	754232.011203	43.482637
3501.668603	754219.860446	43.487642
3501.926019	754198.389328	43.492647
3501.797917	754197.033080	43.497652
3501.745739	754202.054920	43.502657
3501.867885	754185.372797	43.507661
3501.826436	754175.057036	43.512666
3501.531410	754163.994439	43.517671
3501.413864	754172.123205	43.522676
3501.439178	754169.022589	43.527681
3500.982420	754173.714465	43.532685
3501.145590	754172.017757	43.537690
3501.346229	754174.935640	43.542695
3501.595714	754171.947443	43.547700
3501.612634	754171.649901	43.552705
3501.745206	754157.718690	43.557709
3501.599905	754153.170124	43.562714
3501.610971	754140.978258	43.567719
3501.674429	754147.260062	43.572724
3501.779431	754138.641740	43.577729
3501.775523	754132.793055	43.582733
3501.706873	754134.917433	43.587738
3502.178830	754124.078955	43.592743
3501.831679	754122.855243	43.597748
3501.804075	754111.947377	43.602753
3501.703801	754090.777621	43.607757
3501.376959	754088.272717	43.612762
3501.586186	754084.504309	43.617767
3501.371194	754082.965004	43.622772
3501.401103	754087.285933	43.627777
3501.823538	754085.450367	43.632781
3501.371775	754087.143105	43.637786
3501.709267	754080.356231	43.642791
3501.768564	754067.861775	43.647796
3501.336899	754059.081477	43.652801
3501.518166	754052.663081	43.657805
3501.393578	754056.516634	43.662810
3501.312894	754060.854867	43.667815
3501.884576	754055.997540	43.672820
3501.477999	754071.348157	43.677825
3501.762346	754058.081187	43.682829
3501.593160	754055.846553	43.687834
3501.369462	754028.010887	43.692839
3501.679506	754026.291186	43.697844
3501.708465	754022.895008	43.702849
3502.069387	754025.198040	43.707853
3501.474610	754027.060612	43.712858
3501.429169	754014.238351	43.717863
3501.543549	753988.610803	43.722868
3501.589026	753996.763439	43.727873
3501.748594	753988.283870	43.732877
3501.382878	753997.090645	43.737882
3501.433335	754004.898409	43.742887
3501.917937	753999.366489	43.747892
3501.368485	753987.507756	43.752897
3502.084161	753964.784579	43.757901
3501.643788	753966.426409	43.762906
3501.571199	753969.436243	43.767911
3501.768065	753973.780297	43.772916
3501.507052	753984.733542	43.777921
3501.808890	753958.339256	43.782925
3501.785633	753947.479614	43.787930
3502.015003	753941.889237	43.792935
3501.938050	753939.640148	43.797940
3501.204613	753928.596563	43.802945
3501.809770	753917.982728	43.807949
3501.524285	753923.680257	43.812954
3501.749413	753912.585111	43.817959
3501.831749	753901.217337	43.822964
3501.688660	753904.483998	43.827969
3501.727253	753906.296745	43.832973
3501.844784	753897.971107	43.837978
3501.990667	753883.644034	43.842983
3501.676192	753884.381399	43.847988
3501.231532	753884.106845	43.852993
3501.785377	753877.335114	43.857997
3501.664778	753867.965240	43.863002
3501.514762	753851.865594	43.868007
3501.480604	753848.823292	43.873012
3501.313418	753853.076861	43.878017
3501.617685	753842.804887	43.883021
3501.896614	753854.362110	43.888026
3501.411885	753858.173757	43.893031
3501.366249	753853.609418	43.898036
3501.372816	753850.413283	43.903041
3501.938333	753836.905325	43.908045
3501.683349	753830.554925	43.913050
3501.478352	753830.881932	43.918055
3501.377857	753830.258638	43.923060
3501.483417	753825.768959	43.928065
3501.585707	753827.817549	43.933069
3502.021193	753824.357728	43.938074
3501.970740	753804.948953	43.943079
3501.846537	753793.170887	43.948084
3501.752747	753792.251604	43.953089
3501.962343	753775.505694	43.958093
3501.812642	753759.651573	43.963098
3501.724905	753753.619055	43.968103
3501.848690	753751.141900	43.973108
3501.602382	753751.917778	43.978113
3502.056077	753753.124952	43.983117
3501.704798	753735.680121	43.988122
3501.861497	753719.827170	43.993127
3501.939983	753718.782633	43.998132
3501.530004	753718.207708	44.003137
3502.021484	753695.420409	44.008141
3502.175953	753691.021314	44.013146
3501.979891	753687.463524	44.018151
3501.634937	753672.229615	44.023156
3501.708798	753656.831889	44.028161
3501.752467	753654.613010	44.033165
3501.399838	753647.736980	44.038170
3501.771107	753649.448631	44.043175
3502.070457	753653.383602	44.048180
3501.692055	753639.482098	44.053185
3502.072685	753623.348141	44.058189
3501.610170	753615.948525	44.063194
3501.796593	753612.330907	44.068199
3501.626666	753608.080786	44.073204
3501.558403	753602.438357	44.078209
3502.009495	753592.241386	44.083213
3501.819576	753593.008465	44.088218
3502.014123	753587.128310	44.093223
3501.968236	753571.699961	44.098228
3501.883260	753554.901267	44.103233
3501.936047	753546.683655	44.108237
3501.630566	753566.148826	44.113242
3501.696552	753543.771663	44.118247
3501.687804	753523.126649	44.123252
3501.331615	753514.628826	44.128257
3501.525322	753519.170285	44.133261
3501.460200	753528.225595	44.138266
3501.825042	753516.567255	44.143271
3501.956629	753521.216740	44.148276
3501.792626	753505.118497	44.153281
3501.866592	753496.504251	44.158285
3501.686066	753502.087389	44.163290
3501.820749	753500.542452	44.168295
3502.070317	753492.146542	44.173300
3501.508175	753478.568396	44.178305
3501.799941	753471.443985	44.183309
3501.875868	753472.022044	44.188314
3501.675349	753462.516653	44.193319
3501.627613	753443.794689	44.198324
3501.395354	753430.459835	44.203329
3501.837420	753426.949637	44.208333
3501.665900	753437.250666	44.213338
3501.626511	753431.554428	44.218343
3501.991902	753433.660322	44.223348
3501.859621	753420.555614	44.228353
3501.840589	753397.748853	44.233357
3501.996075	753401.804772	44.238362
3501.770885	753396.186711	44.243367
3501.790157	753376.323436	44.248372
3501.557163	753367.953657	44.253377
3502.161959	753372.922540	44.258381
3501.743074	753375.298529	44.263386
3501.922384	753350.936678	44.268391
3501.840255	753337.184905	44.273396
3501.741094	753340.887390	44.278401
3501.710653	753329.536335	44.283405
3501.623253	753328.075237	44.288410
3501.421259	753313.653923	44.293415
3501.504705	753303.563173	44.298420
3501.096934	753299.448367	44.303425
3501.992259	753294.195819	44.308429
3501.753666	753296.150372	44.313434
3501.480603	753299.732584	44.318439
3501.412784	753301.070523	44.323444
3501.175143	753306.367785	44.328449
3501.240740	753296.132335	44.333453
3501.409502	753309.477418	44.338458
3501.419435	753303.920847	44.343463
3501.746519	753299.592847	44.348468
3501.742419	753285.386339	44.353473
3501.478734	753276.333012	44.358477
3501.449636	753279.778777	44.363482
3501.927987	753279.753185	44.368487
3501.776014	753270.190788	44.373492
3501.529258	753272.736542	44.378497
3501.512145	753253.960133	44.383501
3501.404655	753237.606650	44.388506
3501.365255	753245.920895	44.393511
3501.329806	753239.339006	44.398516
3501.396703	753243.113903	44.403521
3501.717479	753241.785621	44.408525
3501.659632	753248.529622	44.413530
3501.543541	753232.767393	44.418535
3501.570161	753242.791928	44.423540
3501.519345	753223.234144	44.428545
3501.579259	753205.133808	44.433549
3501.356445	753212.247755	44.438554
3501.355941	753217.950455	44.443559
3501.370275	753211.459078	44.448564
3501.529503	753215.022916	44.453569
3501.741571	753207.320778	44.458573
3501.434029	753222.166132	44.463578
3501.012053	753209.745405	44.468583
3501.328267	753215.791879	44.473588
3501.184774	753221.615249	44.478593
3501.712718	753216.813358	44.483597
3501.472600	753193.843864	44.488602
3501.656191	753184.523858	44.493607
3501.792837	753187.796277	44.498612
3501.452258	753188.291987	44.503617
3501.646464	753186.590196	44.508621
3501.543199	753186.262240	44.513626
3501.875591	753183.555637	44.518631
3501.583132	753169.983903	44.523636
3501.414194	753162.882044	44.528641
3501.258896	753152.975884	44.533645
3501.587499	753154.350202	44.538650
3501.675350	753154.680620	44.543655
3501.386986	753162.640595	44.548660
3501.257804	753171.313086	44.553665
3501.548515	753161.927145	44.558669
3501.592190	753166.688927	44.563674
3501.483706	753154.071615	44.568679
3501.410110	753146.856514	44.573684
3501.312773	753146.036022	44.578689
3501.696161	753143.616397	44.583693
3501.465543	753147.978622	44.588698
3501.199811	753148.265991	44.593703
3501.390946	753148.334459	44.598708
3501.472364	753148.420079	44.603713
3502.125851	753145.171659	44.608717
3501.332132	753143.673455	44.613722
3501.473881	753126.248377	44.618727
3501.591902	753109.072772	44.623732
3501.541448	753114.144269	44.628737
3501.445045	753103.589741	44.633741
3501.387037	753108.908229	44.638746
3501.591240	753112.563409	44.643751
3501.578270	753119.595483	44.648756
3501.160392	753132.196867	44.653761
3501.449405	753130.578565	44.658765
3501.132693	753135.789991	44.663770
3501.392392	753138.600748	44.668775
3501.340735	753121.599180	44.673780
3501.251339	753125.005285	44.678785
3501.474427	753117.989581	44.683789
3501.422334	753100.988032	44.688794
3501.108668	753096.612591	44.693799
3501.468863	753094.245736	44.698804
3501.439817	753101.083697	44.703809
3501.617624	753088.470676	44.708813
3501.568476	753094.426884	44.713818
3501.207857	753087.797365	44.718823
3501.616638	753102.776795	44.723828
3501.105608	753106.740430	44.728833
3501.495454	753104.516427	44.733837
3501.462376	753111.551652	44.738842
3501.667616	753104.391242	44.743847
3501.562975	753086.709618	44.748852
3501.368008	753074.843103	44.753857
3501.554252	753064.588462	44.758861
3501.353487	753067.815358	44.763866
3501.248849	753073.731097	44.768871
3501.623309	753077.802132	44.773876
3501.643260	753086.303930	44.778881
3501.411376	753079.211827	44.783885
3501.477958	753074.875253	44.788890
3501.392637	753071.004875	44.793895
3501.641320	753052.137223	44.798900
3501.028512	753060.344675	44.803905
3501.583387	753043.641397	44.808909
3501.322792	753053.760257	44.813914
3500.998566	753048.649015	44.818919
3501.197311	753055.353088	44.823924
3501.132173	753067.063701	44.828929
3501.664135	753060.343787	44.833933
3501.719478	753059.253610	44.838938
3501.402138	753063.973573	44.843943
3501.686604	753059.209638	44.848948
3501.555627	753071.471311	44.853953
3501.359085	753067.126704	44.858957
3501.528860	753057.464563	44.863962
3501.445868	753041.942545	44.868967
3501.435655	753034.717423	44.873972
3500.964120	753037.495044	44.878977
3501.383318	753032.513384	44.883981
3501.368883	753032.859797	44.888986
3500.965458	753041.034540	44.893991
3501.323784	753042.404234	44.898996
3501.341789	753043.433836	44.904001
3501.801735	753034.758696	44.909005
3501.883268	753039.858775	44.914010
3501.471247	753047.739885	44.919015
3501.553781	753043.843252	44.924020
3501.330811	753048.646795	44.929025
3501.520859	753031.656389	44.934029
3501.349038	753015.459938	44.939034
3501.627877	753017.579488	44.944039
3501.613012	753012.665668	44.949044
3501.674092	753010.591354	44.954049
3501.516913	753010.566788	44.959053
3501.952082	753011.236212	44.964058
3501.724281	752999.473027	44.969063
3501.643474	752976.084633	44.974068
3501.699485	752985.023372	44.979073
3501.750753	752978.968468	44.984077
3501.286338	752984.989683	44.989082
3501.376839	752980.895123	44.994087
3501.641366	752972.299617	44.999092
3501.420205	752983.100681	45.004097
3501.644427	752957.206446	45.009101
3501.868081	752949.059760	45.014106
3501.610107	752943.446465	45.019111
3501.811094	752944.791612	45.024116
3501.405537	752951.983546	45.029121
3501.656919	752948.699574	45.034125
3502.030342	752935.613245	45.039130
3501.861080	752917.793817	45.044135
3501.760269	752921.300128	45.049140
3501.582299	752913.904458	45.054145
3501.941344	752905.097447	45.059149
3502.054976	752887.086233	45.064154
3501.678040	752872.003096	45.069159
3501.646696	752877.317587	45.074164
3501.729384	752880.106956	45.079169
3502.138236	752863.475248	45.084173
3501.984449	752848.799643	45.089178
3501.517160	752843.956431	45.094183
3501.851595	752840.659427	45.099188
3501.724985	752833.698111	45.104193
3501.633966	752812.375620	45.109197
3501.798940	752817.561140	45.114202
3501.593604	752817.691590	45.119207
3502.016347	752816.986412	45.124212
3501.715267	752795.303402	45.129217
3501.785864	752777.691944	45.134221
3501.220036	752775.863052	45.139226
3501.362820	752779.970475	45.144231
3501.910112	752780.179926	45.149236
3501.657450	752779.678652	45.154241
3501.562733	752775.367111	45.159245
3501.545801	752758.850884	45.164250
3501.623653	752750.333457	45.169255
3501.580596	752744.981389	45.174260
3501.662369	752750.474946	45.179265
3501.590699	752742.030047	45.184269
3501.680370	752746.588264	45.189274
3501.643815	752734.352273	45.194279
3501.798485	752720.808113	45.199284
3501.270404	752713.417801	45.204289
3501.739426	752713.688653	45.209293
3501.767406	752715.749183	45.214298
3501.606719	752717.495058	45.219303
3501.693026	752712.171906	45.224308
3501.437273	752696.872798	45.229313
3501.239451	752671.485978	45.234317
3501.542230	752678.174144	45.239322
3501.473178	752670.613703	45.244327
3501.512459	752671.050064	45.249332
3501.136330	752675.336994	45.254337
3501.812933	752672.183081	45.259341
3501.646827	752678.649559	45.264346
3501.366430	752686.412161	45.269351
3501.330184	752675.306792	45.274356
3501.451058	752688.267212	45.279361
3501.192768	752666.675450	45.284365
3501.515179	752663.822721	45.289370
3501.397857	752647.026943	45.294375
3501.552613	752647.297762	45.299380
3501.255070	752655.259735	45.304385
3501.512758	752641.109349	45.309389
3501.703541	752639.260472	45.314394
3501.187952	752646.224091	45.319399
3501.460453	752652.277879	45.324404
3501.537411	752650.790949	45.329409
3501.355655	752643.100604	45.334413
3501.351090	752645.559555	45.339418
3501.265688	752654.963292	45.344423
3501.462945	752642.788922	45.349428
3501.321821	752626.390130	45.354433
3501.304695	752625.999518	45.359437
3501.211172	752621.048560	45.364442
3501.357379	752625.303032	45.369447
3501.294073	752619.364062	45.374452
3501.320320	752626.636313	45.379457
3501.234245	752619.029314	45.384461
3501.689469	752632.035899	45.389466
3501.401162	752634.637538	45.394471
3501.883254	752626.253428	45.399476
3501.277060	752629.101419	45.404481
3501.171462	752621.202488	45.409485
3501.748539	752627.405343	45.414490
3501.422664	752629.963692	45.419495
3501.676072	752613.011552	45.424500
3501.294728	752611.989572	45.429505
3501.206948	752597.303130	45.434509
3501.233913	752602.264559	45.439514
3501.547812	752609.442697	45.444519
3501.566141	752601.081891	45.449524
3501.052383	752602.637164	45.454529
3501.387191	752597.717561	45.459533
3501.290231	752611.007162	45.464538
3501.063670	752615.123254	45.469543
3501.415560	752612.757542	45.474548
3501.512396	752609.104258	45.479553
3501.512230	752615.004045	45.484557
3501.388369	752611.286934	45.489562
3501.106996	752615.755745	45.494567
3501.417269	752616.198912	45.499572
3501.212211	752630.636156	45.504577
3501.332340	752622.357790	45.509581
3501.482478	752615.254669	45.514586
3501.385069	752602.339663	45.519591
3501.639747	752588.091314	45.524596
3501.502335	752584.376307	45.529601
3501.618541	752574.328571	45.534605
3501.726847	752577.458207	45.539610
3501.337590	752587.892826	45.544615
3501.503003	752588.702792	45.549620
3501.171359	752597.555122	45.554625
3501.424484	752603.022007	45.559629
3501.150711	752595.788476	45.564634
3500.976860	752602.010412	45.569639
3501.463105	752605.425106	45.574644
3501.137410	752602.378681	45.579649
3501.484616	752595.392228	45.584653
3501.485803	752598.587764	45.589658
3501.322668	752587.747917	45.594663
3501.517908	752579.605253	45.599668
3501.530522	752576.555096	45.604673
3501.342985	752569.062233	45.609677
3501.337622	752566.998177	45.614682
3501.447885	752575.830619	45.619687
3501.479994	752569.630869	45.624692
3501.254120	752584.612272	45.629697
3501.422908	752585.667534	45.634701
3501.221719	752574.882781	45.639706
3501.414818	752575.393432	45.644711
3500.854224	752567.467238	45.649716
3501.018977	752580.961807	45.654721
3501.339809	752582.140796	45.659725
3501.151726	752576.614613	45.664730
3501.263506	752575.417211	45.669735
3501.609982	752584.753529	45.674740
3501.501466	752577.444981	45.679745
3501.299070	752581.311491	45.684749
3501.316774	752583.816146	45.689754
3501.287111	752588.393120	45.694759
3501.594165	752583.035364	45.699764
3501.211283	752567.608358	45.704769
3501.595376	752556.781249	45.709773
3501.674736	752547.870027	45.714778
3501.387557	752552.585609	45.719783
3501.339818	752550.479007	45.724788
3501.051043	752566.256920	45.729793
3501.183486	752565.695429	45.734797
3501.390578	752557.452558	45.739802
3501.323712	752557.758025	45.744807
3501.598613	752556.387626	45.749812
3501.087766	752570.479475	45.754817
3501.315267	752540.650038	45.759821
3501.289369	752485.244996	45.764826
3500.841968	752393.424361	45.769831
3500.789248	752244.802368	45.774836
3500.795043	752058.702015	45.779841
3500.541048	751804.733962	45.784845
3500.357184	751504.917701	45.789850
3499.939540	751170.015010	45.794855
3499.642700	750771.836294	45.799860
3498.989953	750336.314327	45.804865
3498.700042	749856.100013	45.809869
3498.312830	749323.976689	45.814874
3497.910537	748749.463071	45.819879
3497.815899	748110.360764	45.824884
3497.052462	747433.816136	45.829889
3496.408335	746695.240713	45.834893
3495.567708	745914.349116	45.839898
3494.925160	745104.452815	45.844903
3493.959962	744243.178677	45.849908
3493.357234	743348.418858	45.854913
3492.813109	742386.286547	45.859917
3491.464408	741378.605593	45.864922
3490.601516	740329.391057	45.869927
3489.622202	739228.080514	45.874932
3488.426464	738080.627422	45.879937
3487.939126	736901.844481	45.884941
3486.438810	735669.564431	45.889946
3485.121702	734390.819376	45.894951
3484.319526	733084.808982	45.899956
3483.077373	731713.901240	45.904961
3481.731946	730304.835722	45.909965
3480.749243	728853.868977	45.914970
3479.010829	727355.923229	45.919975
3478.095604	725815.511039	45.924980
3476.547613	724237.474630	45.929985
3475.211271	722619.882632	45.934989
3473.858596	720944.971791	45.939994
3472.067956	719228.328622	45.944999
3470.474535	717483.510564	45.950004
3468.877498	715704.899004	45.955009
3467.100424	713878.266957	45.960013
3465.871863	712006.928890	45.965018
3463.802409	710100.960893	45.970023
3462.305914	708145.084030	45.975028
3460.310672	706179.105229	45.980033
3458.609248	704158.659168	45.985037
3456.704987	702101.751019	45.990042
3454.690670	700015.964924	45.995047
3452.816717	697889.852493	46.000052
3450.797899	695724.965021	46.005057
3449.005953	693525.873899	46.010061
3446.929205	691294.369406	46.015066
3444.268544	689024.873453	46.020071
3442.211338	686727.387613	46.025076
3440.324905	684403.894542	46.030081
3438.320530	682038.495098	46.035085
3435.758529	679642.889506	46.040090
3433.336296	677212.528905	46.045095
3431.129690	674762.571255	46.050100
3429.008259	672283.040551	46.055105
3426.746108	669765.256057	46.060109
3424.238697	667211.243282	46.065114
3421.892058	664638.113481	46.070119
3419.315315	662032.538664	46.075124
3417.050907	659401.772836	46.080129
3414.306511	656740.349900	46.085133
3412.038607	654041.677600	46.090138
3409.321302	651332.460796	46.095143
3406.788398	648581.319611	46.100148
3404.054559	645811.099998	46.105153
3401.561532	643014.545761	46.110157
3399.273007	640190.000197	46.115162
3395.841704	637340.547364	46.120167
3393.653742	634461.907606	46.125172
3390.793821	631578.560036	46.130177
3388.072363	628643.814528	46.135181
3385.288904	625703.943691	46.140186
3382.421140	622737.179742	46.145191
3379.603615	619729.497176	46.150196
3376.941253	616719.977265	46.155201
3374.027808	613684.346648	46.160205
3370.916088	610620.081342	46.165210
3368.066028	607531.393067	46.170215
3364.959854	604426.704316	46.175220
3362.091571	601298.825336	46.180225
3359.053867	598158.871189	46.185229
3356.365495	594990.283616	46.190234
3352.826474	591814.071551	46.195239
3350.250239	588592.724794	46.200244
3347.100216	585383.841362	46.205249
3344.146545	582138.739648	46.210253
3341.317027	578868.190859	46.215258
3337.974365	575587.582371	46.220263
3334.658977	572273.597380	46.225268
3331.269972	568964.731727	46.230273
3327.992419	565638.377015	46.235277
3324.485444	562280.368467	46.240282
3321.564728	558930.550920	46.245287
3318.315421	555538.732548	46.250292
3315.085699	552152.486079	46.255297
3311.591481	548729.686352	46.260301
3308.502331	545311.550663	46.265306
3304.984960	541885.747812	46.270311
3302.325952	538420.529587	46.275316
3298.346412	534961.819513	46.280321
3295.033144	531488.176829	46.285325
3291.969484	527993.924772	46.290330
3288.104487	524489.348217	46.295335
3285.065234	520977.269818	46.300340
3281.044094	517445.931984	46.305345
3277.903452	513917.979036	46.310349
3274.839718	510360.369616	46.315354
3271.013241	506803.589569	46.320359
3267.508748	503228.057381	46.325364
3264.232888	499656.343944	46.330369
3260.787029	496061.773229	46.335373
3257.000516	492449.668900	46.340378
3253.615143	488842.842719	46.345383
3250.147322	485231.839332	46.350388
3246.021268	481608.421417	46.355393
3242.625991	477980.259431	46.360397
3238.975347	474333.363134	46.365402
3235.303425	470695.251290	46.370407
3232.156205	467034.199157	46.375412
3228.454183	463377.384319	46.380417
3224.923206	459707.709276	46.385421
3221.326366	456032.148424	46.390426
3217.296905	452346.061033	46.395431
3213.982658	448652.918981	46.400436
3210.215308	444967.547393	46.405441
3206.727790	441255.865900	46.410445
3202.841373	437545.686777	46.415450
3198.794265	433836.125447	46.420455
3195.519643	430116.458308	46.425460
3191.840959	426397.317875	46.430465
3187.936209	422674.330045	46.435469
3184.202728	418941.460747	46.440474
3180.576677	415210.340994	46.445479
3176.964821	411462.435615	46.450484
3173.156765	407728.625805	46.455489
3169.159867	403988.990707	46.460493
3165.698412	400240.281113	46.465498
3161.495398	396503.515002	46.470503
3157.872136	392749.265409	46.475508
3153.904076	389009.819694	46.480513
3150.201791	385264.156446	46.485517
3146.457908	381509.515593	46.490522
3142.369553	377774.321511	46.495527
3138.606107	374014.904820	46.500532
3134.797024	370261.581975	46.505537
3130.952937	366513.147514	46.510541
3126.978884	362760.712518	46.515546
3122.932929	359018.968314	46.520551
3119.305567	355271.334773	46.525556
3115.510523	351541.071423	46.530561
3111.358452	347794.466416	46.535565
3107.442656	344055.181280	46.540570
3103.163722	340317.934525	46.545575
3099.357511	336581.540972	46.550580
3095.330814	332870.537749	46.555585
3090.928483	329150.886125	46.560589
3087.448693	325419.874994	46.565594
3083.120661	321715.289414	46.570599
3079.508089	318006.297636	46.575604
3074.944809	314314.315833	46.580609
3070.841314	310616.671019	46.585613
3066.888183	306928.055403	46.590618
3062.724562	303250.168635	46.595623
3059.495620	299565.920793	46.600628
3055.150294	295906.874964	46.605633
3050.965413	292234.945964	46.610637
3047.288115	288572.261878	46.615642
3043.177956	284928.428350	46.620647
3038.892564	281291.123282	46.625652
3034.763131	277646.380846	46.630657
3030.499030	274020.304486	46.635661
3026.324994	270407.016860	46.640666
3022.194278	266793.679315	46.645671
3018.444257	263199.170783	46.650676
3014.129513	259612.040280	46.655681
3009.787879	256038.938742	46.660685
3005.555364	252470.994855	46.665690
3001.407995	248922.154483	46.670695
2996.981424	245370.049710	46.675700
2992.981421	241843.385451	46.680705
2988.744078	238315.128053	46.685709
2984.515957	234810.565585	46.690714
2980.143636	231322.907592	46.695719
2976.268730	227832.147673	46.700724
2971.970883	224360.827419	46.705729
2967.556428	220905.267138	46.710733
2963.358971	217468.149823	46.715738
2958.853680	214038.997701	46.720743
2954.462286	210625.420488	46.725748
2950.295851	207230.873705	46.730753
2945.881101	203838.529636	46.735757
2942.103986	200472.503936	46.740762
2937.433468	197119.393754	46.745767
2932.946767	193773.512903	46.750772
2928.832544	190459.872950	46.755777
2924.799076	187154.843759	46.760781
2920.712196	183855.908015	46.765786
2916.078872	180588.588484	46.770791
2912.269510	177323.038410	46.775796
2907.782152	174071.836850	46.780801
2903.242466	170840.290212	46.785805
2899.376497	167562.556151	46.790810
2894.925198	164323.798346	46.795815
2890.557791	161137.877829	46.800820
2886.617252	157970.096848	46.805825
2881.949602	154819.342771	46.810829
2877.848924	151679.016958	46.815834
2873.480798	148552.373510	46.820839
2869.422974	145452.293686	46.825844
2864.714517	142363.572634	46.830849
2860.837318	139287.625056	46.835853
2856.181547	136236.081136	46.840858
2851.929881	133204.521937	46.845863
2847.928207	130179.897696	46.850868
2843.463170	127184.826378	46.855873
2839.498334	124193.287821	46.860877
2835.472291	121220.853157	46.865882
2831.128037	118273.223777	46.870887
2827.032809	115326.571262	46.875892
2822.747338	112404.708896	46.880897
2818.624928	109495.579912	46.885901
2814.483382	106590.189788	46.890906
2809.836422	103707.267651	46.895911
2805.854546	100846.897612	46.900916
2801.539135	98017.712986	46.905921
2797.265690	95172.771717	46.910925
2793.131105	92360.190411	46.915930
2788.741852	89566.444698	46.920935
2784.507153	86779.757043	46.925940
2780.078750	84028.361788	46.930945
2775.697481	81290.025496	46.935949
2771.778520	78558.359462	46.940954
2767.425682	75859.440064	46.945959
2763.145020	73167.849771	46.950964
2758.867233	70503.854317	46.955969
2754.448927	67846.263858	46.960973
2750.214644	65201.104812	46.965978
2745.518013	62602.268866	46.970983
2741.596493	60003.746877	46.975988
2737.394729	57433.577019	46.980993
2733.008237	54881.702386	46.985997
2728.754929	52340.363654	46.991002
2724.248126	49825.271030	46.996007
2720.114922	47326.110325	47.001012
2715.849286	44842.445724	47.006017
2711.070488	42387.747297	47.011021
2706.840940	39955.115782	47.016026
2702.157398	37543.613964	47.021031
2697.428062	35138.784722	47.026036
2692.897711	32772.016943	47.031041
2688.386424	30435.248793	47.036045
2683.853130	28113.220390	47.041050
2679.157975	25828.236572	47.046055
2674.835278	23562.147967	47.051060
2669.971355	21326.598210	47.056065
2665.423753	19116.980209	47.061069
2660.247733	16934.981135	47.066074
2655.415507	14800.476024	47.071079
2650.723247	12679.369521	47.076084
2645.673567	10605.663973	47.081089
2640.064365	8571.508697	47.086093
2632.612537	6621.090379	47.091098
2622.386673	4813.738464	47.096103
2611.413820	3102.781219	47.101108
2598.577494	1554.367858	47.106113
2579.632616	313.455410	47.111117
2526.553336	198.556314	47.116122
2485.305299	216.623391	47.121127
2467.952733	218.499491	47.126132
2467.907216	209.951489	47.131137
2476.862980	207.933581	47.136141
2489.239727	217.824095	47.141146
2498.879838	221.644095	47.146151
2504.807630	213.325993	47.151156
2506.018335	217.274992	47.156161
2505.008566	209.175231	47.161165
2502.109129	202.586007	47.166170
2498.152602	209.374530	47.171175
2494.277753	211.078569	47.176180
2491.399850	207.754272	47.181185
2488.070287	205.133407	47.186189
2485.678807	201.312225	47.191194
2482.829521	202.666004	47.196199
2479.550068	204.340186	47.201204
2477.182503	198.050599	47.206209
2473.888551	206.304766	47.211213
2470.607828	196.886573	47.216218
2467.743490	202.675310	47.221223
2464.742621	201.005986	47.226228
2461.509220	192.779508	47.231233
2458.122131	190.588451	47.236237
2455.316892	193.172423	47.241242
2451.703379	187.973134	47.246247
2448.894965	187.517115	47.251252
2445.511958	177.554936	47.256257
2441.946480	185.190326	47.261261
2439.166046	178.535056	47.266266
2435.179414	185.277676	47.271271
2431.943951	182.920534	47.276276
2428.385615	186.270918	47.281281
2425.367821	188.268027	47.286285
2422.311403	179.874672	47.291290
2418.715245	183.620133	47.296295
2415.567274	184.815000	47.301300
2412.252389	185.555070	47.306305
2408.905047	191.384574	47.311309
2405.426249	182.313788	47.316314
2401.658378	177.448729	47.321319
2398.678245	175.209848	47.326324
2394.784919	180.061702	47.331329
2391.478289	192.715655	47.336333
2388.604312	179.048059	47.341338
2384.721502	184.069121	47.346343
2381.579777	179.836970	47.351348
2378.092922	181.679672	47.356353
2374.801919	184.425079	47.361357
2371.831291	178.675979	47.366362
2367.761636	183.738932	47.371367
2364.235826	179.709248	47.376372
2360.253024	176.326885	47.381377
2357.419772	187.967113	47.386381
2354.744652	177.764506	47.391386
2350.933160	195.043941	47.396391
2347.081192	177.932030	47.401396
2343.946306	185.420985	47.406401
2340.311946	193.497467	47.411405
2337.393451	173.853965	47.416410
2333.441718	177.908187	47.421415
2330.219773	180.196695	47.426420
2326.451981	183.861462	47.431425
2322.416250	177.472219	47.436429
2319.388928	176.294314	47.441434
2315.978255	184.902138	47.446439
2313.042530	178.673014	47.451444
2309.270075	182.711852	47.456449
2306.160875	181.591054	47.461453
2302.846640	169.615443	47.466458
2299.119225	172.473439	47.471463
2295.224747	183.200819	47.476468
2292.085326	174.352244	47.481473
2288.560826	178.845860	47.486477
2285.234820	170.121396	47.491482
2281.260349	165.136843	47.496487
2278.028747	167.461678	47.501492
2274.686528	169.788001	47.506497
2271.040241	177.135505	47.511501
2267.820532	168.998718	47.516506
2264.366144	173.361144	47.521511
2260.767898	173.500160	47.526516
2257.307358	169.994999	47.531521
2253.598307	179.351896	47.536525
2250.824234	167.415189	47.541530
2246.928512	170.653886	47.546535
2243.223914	178.402842	47.551540
2239.967971	165.462649	47.556545
2236.345293	177.530129	47.561549
2232.735279	170.900309	47.566554
2229.262628	178.198511	47.571559
2226.056125	173.967055	47.576564
2222.751303	169.924995	47.581569
2219.286494	170.973327	47.586573
2215.537867	163.602710	47.591578
2211.746137	172.285989	47.596583
2208.668245	167.755997	47.601588
2205.358636	173.823261	47.606593
2201.500857	180.473020	47.611597
2198.285693	171.832490	47.616602
2194.326687	167.753583	47.621607
2191.131731	165.763517	47.626612
2187.759141	171.226847	47.631617
2184.032415	172.774929	47.636621
2181.281468	168.867697	47.641626
2177.368393	171.587094	47.646631
2173.735606	166.935117	47.651636
2170.743500	165.429030	47.656641
2166.698263	168.697475	47.661645
2163.277815	167.840560	47.666650
2159.235552	170.213168	47.671655
2156.073627	172.166453	47.676660
2152.989163	160.689653	47.681665
2149.049046	162.138251	47.686669
2146.070764	166.201581	47.691674
2142.412393	164.331495	47.696679
2138.537606	163.017310	47.701684
2135.351735	156.226255	47.706689
2131.675578	165.574865	47.711693
2128.616481	156.973227	47.716698
2124.998625	163.572809	47.721703
2121.610945	160.957999	47.726708
2117.801161	166.559357	47.731713
2114.357371	161.039407	47.736717
2111.245610	158.957253	47.741722
2107.284678	158.903122	47.746727
2103.922644	161.495193	47.751732
2100.369280	158.757613	47.756737
2096.651678	155.928670	47.761741
2093.709659	155.262686	47.766746
2090.111374	159.451512	47.771751
2086.716616	156.053183	47.776756
2083.144069	157.997968	47.781761
2079.323774	160.838926	47.786765
2076.058488	153.348449	47.791770
2072.333970	159.993207	47.796775
2068.688480	155.691285	47.801780
2065.392954	146.572993	47.806785
2061.796108	156.640060	47.811789
2058.695124	154.040527	47.816794
2055.294543	164.149658	47.821799
2051.901228	155.502264	47.826804
2048.006594	152.068266	47.831809
2044.593912	165.912654	47.836813
2041.264538	148.070564	47.841818
2037.418123	156.528314	47.846823
2034.322174	157.569608	47.851828
2030.903747	156.462476	47.856833
2026.791354	153.236572	47.861837
2023.768932	150.577300	47.866842
2019.898690	159.636755	47.871847
2016.443738	152.286713	47.876852
2012.988668	151.786455	47.881857
2009.472029	161.407538	47.886861
2006.371084	150.711690	47.891866
2002.472519	155.934653	47.896871
1999.195518	151.685834	47.901876
1995.609829	157.267980	47.906881
1992.065517	157.363843	47.911885
1988.476716	152.939182	47.916890
1984.929607	166.665406	47.921895
1981.664300	161.237804	47.926900
1978.262163	156.106870	47.931905
1974.701252	154.873351	47.936909
1971.351384	149.003392	47.941914
1967.819709	148.031065	47.946919
1964.016968	158.456252	47.951924
1960.423675	157.028481	47.956929
1956.973431	159.090214	47.961933
1953.881890	154.951599	47.966938
1950.346154	150.547124	47.971943
1946.628590	148.101059	47.976948
1943.167981	147.076490	47.981953
1939.713916	152.574777	47.986957
1936.711331	146.941563	47.991962
1932.914137	150.848338	47.996967
1929.156604	157.890622	48.001972
1925.606270	151.878035	48.006977
1921.828394	156.971403	48.011981
1918.940127	150.668550	48.016986
1915.052988	154.867826	48.021991
1911.632988	155.969354	48.026996
1908.452436	143.577521	48.032001
1904.498068	154.817414	48.037005
1901.268250	141.965043	48.042010
1897.451019	156.021459	48.047015
1893.885680	147.720600	48.052020
1890.755254	149.542474	48.057025
1887.275967	151.305042	48.062029
1883.765496	143.207581	48.067034
1880.387167	149.475505	48.072039
1876.791362	149.835737	48.077044
1873.140549	146.411113	48.082049
1869.568278	150.194123	48.087053
1866.312711	150.055012	48.092058
1862.787484	153.106139	48.097063
1859.237390	149.267112	48.102068
1855.973003	144.130491	48.107073
1851.899970	139.110924	48.112077
1848.724841	138.892791	48.117082
1845.468272	140.531930	48.122087
1841.442595	147.749080	48.127092
1838.103435	145.455818	48.132097
1834.567211	150.217156	48.137101
1831.565480	144.121922	48.142106
1827.779529	136.665566	48.147111
1824.016532	153.159170	48.152116
1820.624273	142.853847	48.157121
1817.186862	149.776460	48.162125
1813.923720	145.180678	48.167130
1810.387336	148.037408	48.172135
1806.660518	136.094952	48.177140
1803.372922	141.760218	48.182145
1799.492046	149.793143	48.187149
1796.167494	140.391590	48.192154
1792.618789	142.073299	48.197159
1789.195020	136.911025	48.202164
1785.588690	141.933292	48.207169
1781.962921	153.482473	48.212173
1778.610236	151.542535	48.217178
1774.963923	156.792535	48.222183
1771.576245	144.531252	48.227188
1768.422470	145.578506	48.232193
1764.792077	146.184642	48.237197
1761.438511	141.789698	48.242202
1757.599155	150.578627	48.247207
1754.142520	147.778577	48.252212
1750.871267	147.933032	48.257217
1746.863023	150.721254	48.262221
1743.621555	133.090195	48.267226
1740.378246	146.079193	48.272231
1736.998273	147.225134	48.277236
1733.804397	142.068030	48.282241
1729.401495	150.461093	48.287245
1726.180607	139.388650	48.292250
1722.650431	145.756312	48.297255
1719.064822	138.879271	48.302260
1715.864311	139.744024	48.307265
1712.064134	140.221721	48.312269
1708.656988	141.653506	48.317274
1705.271889	144.546705	48.322279
1701.763682	141.001749	48.327284
1698.174894	138.598902	48.332289
1694.503988	141.717173	48.337293
1691.017696	139.279305	48.342298
1687.450000	134.443324	48.347303
1684.309359	150.690854	48.352308
1681.041257	141.517801	48.357313
1677.324306	139.087562	48.362317
1673.728527	140.248314	48.367322
1670.064156	141.536864	48.372327
1666.269583	143.279241	48.377332
1663.152654	139.995776	48.382337
1659.620591	136.672877	48.387341
1656.061323	143.307709	48.392346
1652.892902	141.623723	48.397351
1649.307490	135.869848	48.402356
1645.817255	134.163463	48.407361
1642.164725	134.811072	48.412365
1638.742959	133.565387	48.417370
1635.172591	140.610098	48.422375
1631.694096	139.259395	48.427380
1628.548533	129.804592	48.432385
1624.645439	135.926914	48.437389
1621.205557	129.950954	48.442394
1617.104349	124.163926	48.447399
1613.978066	125.909296	48.452404
1610.934575	131.751547	48.457409
1606.988355	133.932143	48.462413
1603.871879	131.072584	48.467418
1600.182395	126.192424	48.472423
1596.359030	128.780915	48.477428
1593.212886	130.636971	48.482433
1589.414349	134.003048	48.487437
1585.849606	132.773432	48.492442
1582.365399	134.967149	48.497447
1578.897288	128.011668	48.502452
1575.285282	129.532507	48.507457
1572.030185	136.682919	48.512461
1568.896253	135.173902	48.517466
1565.300697	136.147989	48.522471
1561.620180	129.399770	48.527476
1558.219152	134.291893	48.532481
1554.356689	140.056693	48.537485
1551.380085	135.390848	48.542490
1547.773193	138.015080	48.547495
1544.008239	129.492511	48.552500
1540.367705	133.919074	48.557505
1536.696571	134.367147	48.562509
1533.747508	133.072822	48.567514
1530.275053	128.636461	48.572519
1526.561247	131.321726	48.577524
1523.233110	130.387303	48.582529
1519.488505	144.324865	48.587533
1516.174671	130.577792	48.592538
1512.502752	138.204761	48.597543
1509.020129	138.379721	48.602548
1505.877320	129.706005	48.607553
1502.184775	129.654390	48.612557
1498.486675	130.030765	48.617562
1495.068919	132.818403	48.622567
1491.335218	131.577301	48.627572
1488.227781	133.981002	48.632577
1484.770243	127.169441	48.637581
1481.043959	126.164470	48.642586
1477.506775	127.129451	48.647591
1473.807525	134.574041	48.652596
1470.474133	129.837518	48.657601
1467.147689	135.955055	48.662605
1463.341111	122.376892	48.667610
1460.052667	138.321707	48.672615
1456.688337	129.328334	48.677620
1453.247383	126.709446	48.682625
1449.343934	129.278885	48.687629
1445.884550	123.128874	48.692634
1442.175119	130.445348	48.697639
1439.049592	133.320144	48.702644
1435.930766	126.778297	48.707649
1432.108532	138.307688	48.712653
1428.559622	127.213953	48.717658
1425.024931	122.815851	48.722663
1421.738429	124.415509	48.727668
1418.192798	122.246466	48.732673
1414.472707	129.393770	48.737677
1410.957402	116.526202	48.742682
1407.326018	125.883800	48.747687
1403.908977	125.912486	48.752692
1400.729785	116.257395	48.757697
1396.829965	128.235545	48.762701
1393.276187	123.764510	48.767706
1390.197899	128.277122	48.772711
1386.512871	119.890818	48.777716
1383.327170	121.193128	48.782721
1379.256490	128.964813	48.787725
1375.665550	119.905707	48.792730
1372.360333	125.064466	48.797735
1368.896632	124.929621	48.802740
1365.995100	115.003284	48.807745
1361.835727	127.996535	48.812749
1358.387378	118.684157	48.817754
1354.729966	122.740087	48.822759
1351.388992	121.007281	48.827764
1348.131423	114.601088	48.832769
1344.576458	124.544706	48.837773
1340.896398	122.969390	48.842778
1337.446901	131.339895	48.847783
1333.768722	136.193210	48.852788
1330.026067	127.553350	48.857793
1326.746360	125.918532	48.862797
1323.307698	126.051873	48.867802
1319.828204	126.311832	48.872807
1316.672062	125.413832	48.877812
1313.619521	121.750241	48.882817
1309.528837	126.044859	48.887821
1306.091568	117.917208	48.892826
1302.255543	132.005172	48.897831
1298.618983	127.442726	48.902836
1295.822486	116.765962	48.907841
1291.857574	135.445852	48.912845
1288.351046	126.471646	48.917850
1285.005420	127.549079	48.922855
1281.504839	127.214388	48.927860
1278.053454	121.904773	48.932865
1273.924480	132.488780	48.937869
1270.583191	126.222272	48.942874
1267.274213	121.526299	48.947879
1263.631199	123.763964	48.952884
1260.603018	118.299519	48.957889
1256.773187	123.844166	48.962893
1253.400387	116.807461	48.967898
1250.219958	119.440961	48.972903
1246.655129	126.133729	48.977908
1243.086748	117.166067	48.982913
1239.516323	124.068526	48.987917
1235.826166	125.702960	48.992922
1231.875983	130.181262	48.997927
1228.746382	115.598713	49.002932
1225.610836	112.568259	49.007937
1221.468948	117.396121	49.012941
1218.186296	117.761346	49.017946
1214.768636	122.257529	49.022951
1211.500254	124.955432	49.027956
1208.037374	116.483811	49.032961
1204.476577	118.300491	49.037965
1200.890638	106.621033	49.042970
1197.403779	114.516517	49.047975
1193.691919	115.300129	49.052980
1190.047067	122.521145	49.057985
1186.978488	124.032977	49.062989
1183.819423	122.255933	49.067994
1180.117847	120.231620	49.072999
1175.898145	120.193051	49.078004
1172.482427	115.735296	49.083009
1169.059913	124.550885	49.088013
1165.829615	115.128523	49.093018
1161.967888	116.764534	49.098023
1158.537562	126.445076	49.103028
1155.227961	116.671292	49.108033
1152.165182	124.459271	49.113037
1148.618956	123.673018	49.118042
1144.761905	114.877148	49.123047
1141.284086	123.429314	49.128052
1137.789419	115.294903	49.133057
1134.541938	128.708623	49.138061
1131.209972	124.731327	49.143066
1127.403095	112.925134	49.148071
1123.424303	119.657436	49.153076
1119.910405	114.772136	49.158081
1116.667376	122.003033	49.163085
1113.163817	114.366748	49.168090
1109.725514	117.464617	49.173095
1106.205712	119.246439	49.178100
1103.025596	121.493948	49.183105
1099.082716	123.376812	49.188109
1095.871202	114.413459	49.193114
1092.060219	109.546209	49.198119
1088.470758	116.182766	49.203124
1085.140704	111.176947	49.208129
1081.388158	119.291237	49.213133
1078.560518	121.157695	49.218138
1075.148981	115.898873	49.223143
1071.075100	121.959532	49.228148
1068.075889	109.976296	49.233153
1063.980843	124.130183	49.238157
1060.669301	121.731633	49.243162
1057.185966	121.302572	49.248167
1053.580705	121.500058	49.253172
1050.304437	114.040190	49.258177
1046.524364	115.926059	49.263181
1043.347681	117.046725	49.268186
1039.863032	112.501736	49.273191
1036.465874	128.530088	49.278196
1032.879870	114.673999	49.283201
1028.867535	116.238727	49.288205
1025.651726	115.055931	49.293210
1022.126425	109.593477	49.298215
1018.338418	117.175488	49.303220
1015.306139	112.056633	49.308225
1011.527567	111.376416	49.313229
1008.318876	109.876129	49.318234
1004.678296	115.577895	49.323239
1001.031272	121.790050	49.328244
997.901731	111.997635	49.333249
994.182775	117.385803	49.338253
990.854644	111.180629	49.343258
986.954656	117.011605	49.348263
983.564976	122.000201	49.353268
980.333069	103.118331	49.358273
976.475409	115.700615	49.363277
973.197701	113.170247	49.368282
969.489368	116.329426	49.373287
966.027386	117.713093	49.378292
962.915587	107.152272	49.383297
959.438426	114.967211	49.388301
955.775013	106.413206	49.393306
952.408717	115.264343	49.398311
948.439506	121.726283	49.403316
944.867414	115.492885	49.408321
941.595061	121.383796	49.413325
937.914080	117.992747	49.418330
934.463101	116.555733	49.423335
930.869052	119.801438	49.428340
927.675875	116.552317	49.433345
923.950956	120.910037	49.438349
920.350722	114.045127	49.443354
917.081824	117.695515	49.448359
913.290298	119.409218	49.453364
910.189962	115.136306	49.458369
906.741547	118.137748	49.463373
903.264596	111.500321	49.468378
899.594815	118.573468	49.473383
895.946576	123.219754	49.478388
892.913093	118.987001	49.483393
889.155163	114.336165	49.488397
885.394143	109.106835	49.493402
881.977919	106.335594	49.498407
878.642308	111.872587	49.503412
875.020007	111.092023	49.508417
871.382111	114.044052	49.513421
868.300959	114.067789	49.518426
864.774701	123.738121	49.523431
860.771572	114.819726	49.528436
857.657265	113.801433	49.533441
854.142967	111.130983	49.538445
850.572952	109.241231	49.543450
846.971810	107.232967	49.548455
843.299120	121.298636	49.553460
840.124328	107.314982	49.558465
836.871135	118.347298	49.563469
832.701423	112.264479	49.568474
829.160024	116.824454	49.573479
825.277717	113.328934	49.578484
822.781392	108.724187	49.583489
819.074513	114.040920	49.588493
815.618265	112.538336	49.593498
812.085411	117.843640	49.598503
808.038500	119.714437	49.603508
805.077986	116.112546	49.608513
801.324877	118.873829	49.613517
798.096390	120.954999	49.618522
794.459656	107.110143	49.623527
790.678850	115.244772	49.628532
787.486376	108.119913	49.633537
784.075588	105.110573	49.638541
780.339727	118.967847	49.643546
776.886365	110.004535	49.648551
773.745077	122.879672	49.653556
770.202238	103.087963	49.658561
766.476217	124.059133	49.663565
762.897103	111.584694	49.668570
759.684826	118.665339	49.673575
755.865812	123.091639	49.678580
752.587340	107.257607	49.683585
748.865715	116.211902	49.688589
745.143242	113.210256	49.693594
741.713204	111.365068	49.698599
738.052977	119.404901	49.703604
735.074609	110.920893	49.708609
731.274291	111.626784	49.713613
728.397796	108.521139	49.718618
724.597789	100.672021	49.723623
720.503479	110.393381	49.728628
717.470998	115.462166	49.733633
713.982738	114.271525	49.738637
710.304947	110.636461	49.743642
706.869002	111.456147	49.748647
703.148059	117.287662	49.753652
699.955067	103.208848	49.758657
696.136892	109.514344	49.763661
692.628418	117.622177	49.768666
689.059646	109.059802	49.773671
685.914611	111.491778	49.778676
682.836305	107.614143	49.783681
679.090638	115.116870	49.788685
675.490634	122.558824	49.793690
672.079418	119.897612	49.798695
668.216669	115.639783	49.803700
664.813637	115.805748	49.808705
661.287654	113.086583	49.813709
657.939882	113.636209	49.818714
654.344142	111.155768	49.823719
650.385555	115.388825	49.828724
647.153536	108.276544	49.833729
643.740485	111.541462	49.838733
640.330703	110.104438	49.843738
637.133310	109.415615	49.848743
633.517195	118.290148	49.853748
630.062809	105.229923	49.858753
626.238650	111.954006	49.863757
622.439516	114.409347	49.868762
619.444634	109.667604	49.873767
615.385745	113.967004	49.878772
612.325449	108.953928	49.883777
608.955404	108.330121	49.888781
605.509737	109.676560	49.893786
601.461702	111.345135	49.898791
597.757140	117.164631	49.903796
594.733632	110.146268	49.908801
591.082900	116.175639	49.913805
588.143930	110.748093	49.918810
584.553184	105.950986	49.923815
580.870567	106.388564	49.928820
577.475283	115.548074	49.933825
573.809407	117.628217	49.938829
569.966582	104.862980	49.943834
566.751738	108.612583	49.948839
563.061555	103.315358	49.953844
559.558416	104.547427	49.958849
556.067099	108.514344	49.963853
552.665666	105.421371	49.968858
549.280557	104.227296	49.973863
545.934942	110.234203	49.978868
542.545615	107.376624	49.983873
538.812837	102.522688	49.988877
535.143391	116.606914	49.993882
531.707218	101.509554	49.998887
527.894867	118.931842	50.003892
524.722656	108.481912	50.008897
521.264166	107.827696	50.013901
518.061741	101.217048	50.018906
514.462145	105.023764	50.023911
510.456133	115.838708	50.028916
506.943573	99.895933	50.033921
503.668315	112.475727	50.038925
499.936357	104.429393	50.043930
496.695832	96.394680	50.048935
492.990654	111.636137	50.053940
489.860689	108.592421	50.058945
486.541070	110.637347	50.063949
482.615894	114.067957	50.068954
479.200694	105.737896	50.073959
475.533257	107.669622	50.078964
472.292934	97.445529	50.083969
468.505919	108.624823	50.088973
464.785352	106.648076	50.093978
461.352068	92.508942	50.098983
457.892068	109.553342	50.103988
454.736521	95.111276	50.108993
451.492238	104.671116	50.113997
447.802806	103.005882	50.119002
444.045982	105.492632	50.124007
440.253112	109.456202	50.129012
437.177293	101.079332	50.134017
433.928954	111.367493	50.139021
430.030244	101.148464	50.144026
426.839310	96.216038	50.149031
423.108131	106.272939	50.154036
419.812469	107.364992	50.159041
416.157540	96.364294	50.164045
412.281758	108.082701	50.169050
409.073486	103.561127	50.174055
405.397867	105.737775	50.179060
402.113529	94.660054	50.184065
398.508304	103.172277	50.189069
394.969384	104.349900	50.194074
391.854325	105.976832	50.199079
387.876658	102.237020	50.204084
384.390708	96.328911	50.209089
381.105325	97.071350	50.214093
377.458143	103.182494	50.219098
374.122783	94.887438	50.224103
370.938930	94.364273	50.229108
367.423794	93.032446	50.234113
363.320216	108.614758	50.239117
359.709776	104.026484	50.244122
356.599648	98.622675	50.249127
353.021041	108.222259	50.254132
349.650228	98.135723	50.259137
345.819271	107.287611	50.264141
342.363597	108.306679	50.269146
338.910373	106.050824	50.274151
335.418354	110.353293	50.279156
332.374708	108.602768	50.284161
329.003126	106.561922	50.289165
324.905130	103.973631	50.294170
321.285439	97.153177	50.299175
317.796753	107.665681	50.304180
313.969346	102.352101	50.309185
310.996362	110.176850	50.314189
307.788866	108.034377	50.319194
304.201374	101.493629	50.324199
300.644157	115.772315	50.329204
297.489796	99.466652	50.334209
293.241360	107.212787	50.339213
289.914314	98.672851	50.344218
286.303315	102.187204	50.349223
282.624812	102.013644	50.354228
279.577446	105.031576	50.359233
275.953729	100.192316	50.364237
272.202814	104.044973	50.369242
268.791283	98.862424	50.374247
265.343803	101.661460	50.379252
262.134059	103.781003	50.384257
258.838893	103.227858	50.389261
255.132628	102.448045	50.394266
251.457717	92.171911	50.399271
247.892496	101.152487	50.404276
244.061076	95.194155	50.409281
240.581868	105.806438	50.414285
237.367488	99.741955	50.419290
234.263509	101.797482	50.424295
230.262608	107.046589	50.429300
227.215560	102.455539	50.434305
223.276295	101.161738	50.439309
219.786019	108.865065	50.444314
216.681656	104.937904	50.449319
212.739456	103.277567	50.454324
209.368848	99.515508	50.459329
205.778761	103.254409	50.464333
202.034919	93.916093	50.469338
198.925477	97.057671	50.474343
195.686819	106.543936	50.479348
192.285511	94.741144	50.484353
188.469481	105.279657	50.489357
184.604682	101.379890	50.494362
181.188008	92.556651	50.499367
178.017264	103.620508	50.504372
174.291330	105.488750	50.509377
170.885161	104.579700	50.514381
167.261869	104.615842	50.519386
163.765479	101.835303	50.524391
160.258668	104.988528	50.529396
156.899413	102.661078	50.534401
153.120851	111.153085	50.539405
149.853822	92.128464	50.544410
146.769167	93.734897	50.549415
142.902146	92.701903	50.554420
139.579301	94.383620	50.559425
135.845620	101.612569	50.564429
132.143471	97.883502	50.569434
129.030150	92.100631	50.574439
125.158534	100.958404	50.579444
121.502175	92.805504	50.584449
118.315511	89.966971	50.589453
114.745212	92.247457	50.594458
111.654070	100.419803	50.599463
107.678166	99.103322	50.604468
104.064983	93.496852	50.609473
100.642638	104.840598	50.614477
97.224001	90.205806	50.619482
94.122827	91.084007	50.624487
90.226027	93.937683	50.629492
86.619635	96.005534	50.634497
83.198477	102.578090	50.639501
79.386027	95.601287	50.644506
76.350603	94.137474	50.649511
72.472847	101.901554	50.654516
69.184527	94.886933	50.659521
66.005097	97.533313	50.664525
62.317287	96.965830	50.669530
58.764075	98.886153	50.674535
55.134605	100.619106	50.679540
51.916973	92.549365	50.684545
48.085330	96.848197	50.689549
44.546286	92.843677	50.694554
41.194506	95.852431	50.699559
37.475184	95.501871	50.704564
34.207679	93.539753	50.709569
30.783994	96.268708	50.714573
27.311688	92.054419	50.719578
23.810779	90.442092	50.724583
20.161910	94.500324	50.729588
16.900571	106.325077	50.734593
13.056876	98.116157	50.739597
9.306790	102.639513	50.744602
6.233856	90.389892	50.749607
2.806098	92.806279	50.754612