Tue Jun 08 17:02:17 2021

Number of Points = 14581

Depth (nm)	Load (N)	Time (s)
0.036298	99.701863	0.000000
0.067460	77.094437	0.005005
-1.058458	51.674970	0.010010
-2.669327	10.530128	0.015014
-6.868233	-2.076572	0.020019
-12.379601	6.686417	0.025024
-16.977895	-6.454116	0.030029
-21.491520	-1.996394	0.035034
-25.523640	3.163455	0.040038
-29.261378	1.429735	0.045043
-33.269693	7.940552	0.050048
-36.582723	0.139546	0.055053
-40.107067	9.715987	0.060058
-43.809501	-1.803119	0.065062
-47.787581	6.633841	0.070067
-51.644443	4.274031	0.075072
-54.993214	-0.219473	0.080077
-59.198616	10.960639	0.085082
-62.874364	4.130868	0.090086
-66.545276	5.460909	0.095091
-70.676544	5.583532	0.100096
-73.846167	1.036430	0.105101
-77.833147	10.087137	0.110106
-81.796954	8.655894	0.115110
-85.345060	-2.618866	0.120115
-89.440866	4.476169	0.125120
-93.223504	-5.858423	0.130125
-97.034371	5.100122	0.135130
-100.810068	6.586308	0.140134
-103.906016	3.757398	0.145139
-108.104909	0.967639	0.150144
-111.676339	0.095936	0.155149
-115.224922	6.165242	0.160154
-119.334655	5.360200	0.165158
-123.043763	8.628548	0.170163
-126.774585	9.235144	0.175168
-130.242734	0.312605	0.180173
-134.280174	-1.798680	0.185178
-138.473188	0.593125	0.190182
-141.950621	-7.822579	0.195187
-145.932268	5.304616	0.200192
-149.860484	6.251378	0.205197
-153.593379	9.445282	0.210202
-156.762361	4.012401	0.215206
-160.696917	-2.175699	0.220211
-164.976148	1.929746	0.225216
-168.317050	-6.010438	0.230221
-171.869627	3.249636	0.235226
-175.607406	5.133563	0.240230
-179.655097	2.261893	0.245235
-183.735717	0.159243	0.250240
-187.021867	-0.286095	0.255245
-190.668668	-3.146776	0.260250
-194.328707	2.812630	0.265254
-198.280777	-2.078967	0.270259
-202.456517	11.545346	0.275264
-205.639225	9.092547	0.280269
-209.715227	4.774807	0.285274
-213.630999	3.801595	0.290278
-217.010978	-0.579067	0.295283
-220.837433	1.705736	0.300288
-224.674272	-0.776163	0.305293
-228.578549	8.220216	0.310298
-232.125589	9.229164	0.315302
-236.183894	4.962094	0.320307
-240.184509	11.613460	0.325312
-243.295583	1.150797	0.330317
-247.243311	9.470612	0.335322
-251.213024	0.233968	0.340326
-254.599953	-7.357219	0.345331
-258.800076	4.366052	0.350336
-262.260598	-4.048108	0.355341
-266.087023	-3.786948	0.360346
-269.560042	2.801180	0.365350
-273.690390	-2.707881	0.370355
-277.482844	0.506992	0.375360
-280.938721	0.020182	0.380365
-284.970859	11.103656	0.385370
-288.706493	6.619853	0.390374
-291.980238	5.789991	0.395379
-296.235928	12.626066	0.400384
-300.195850	8.191796	0.405389
-303.697255	15.684760	0.410394
-307.813987	9.665005	0.415398
-311.414932	-3.451276	0.420403
-315.232373	11.086992	0.425408
-318.513598	6.382386	0.430413
-322.634087	5.320052	0.435418
-326.413832	12.030306	0.440422
-329.812797	4.491762	0.445427
-333.853964	9.596190	0.450432
-337.160110	0.366587	0.455437
-340.941534	4.677307	0.460442
-345.395152	8.671919	0.465446
-348.834634	-1.459604	0.470451
-353.063386	5.707795	0.475456
-356.391567	4.227364	0.480461
-360.085921	6.692897	0.485466
-364.026735	8.802846	0.490470
-367.174250	4.906599	0.495475
-371.089644	10.293409	0.500480
-375.029856	1.013145	0.505485
-378.963324	5.938488	0.510490
-382.537846	7.167780	0.515494
-386.252944	-4.084372	0.520499
-390.637473	6.310476	0.525504
-394.396028	-4.009805	0.530509
-398.121887	3.673292	0.535514
-401.890476	12.641794	0.540518
-405.420383	3.237490	0.545523
-409.056600	5.498893	0.550528
-412.889598	0.606409	0.555533
-416.559038	3.931336	0.560538
-420.485171	12.622953	0.565542
-423.858456	-1.250649	0.570547
-427.897293	7.553457	0.575552
-431.539448	-5.051990	0.580557
-435.444004	-0.095248	0.585562
-438.889984	7.507500	0.590566
-442.815168	-2.660209	0.595571
-446.956722	2.751646	0.600576
-450.274836	-7.987932	0.605581
-453.871729	0.353952	0.610586
-458.458026	5.465173	0.615590
-461.793645	-2.044258	0.620595
-465.542067	7.260673	0.625600
-469.248386	-1.747804	0.630605
-473.025902	1.748462	0.635610
-476.600543	3.936200	0.640614
-480.498205	-2.849200	0.645619
-484.406408	7.112718	0.650624
-487.842732	-4.149273	0.655629
-491.711036	-1.055017	0.660634
-495.678371	7.886472	0.665638
-499.026295	-8.919748	0.670643
-503.270390	0.358153	0.675648
-507.068213	-0.302295	0.680653
-510.661425	-0.493803	0.685658
-514.347266	9.188031	0.690662
-517.979130	2.023137	0.695667
-521.865323	0.385568	0.700672
-525.534081	-1.397061	0.705677
-529.383994	-5.060964	0.710682
-533.215481	2.757982	0.715686
-536.638814	-3.370250	0.720691
-540.990889	6.221456	0.725696
-544.794087	3.500796	0.730701
-548.459453	0.210610	0.735706
-552.001585	8.238852	0.740710
-555.571203	-9.009240	0.745715
-559.609053	1.797944	0.750720
-563.439026	-12.063470	0.755725
-566.874241	-0.850513	0.760730
-570.598697	2.492660	0.765734
-574.303455	3.566437	0.770739
-578.708414	-5.138122	0.775744
-582.304538	-4.981334	0.780749
-586.351158	-1.616419	0.785754
-589.756363	-1.015973	0.790758
-593.219252	-1.950512	0.795763
-597.070926	4.192071	0.800768
-600.886232	7.700453	0.805773
-604.704962	6.317809	0.810778
-608.737656	5.993388	0.815782
-612.035496	-13.389679	0.820787
-616.120955	5.234617	0.825792
-619.486969	4.170194	0.830797
-623.373771	5.099605	0.835802
-627.241790	4.509329	0.840806
-630.924838	1.384473	0.845811
-635.050548	-3.177726	0.850816
-638.643998	-1.094388	0.855821
-642.231000	3.461875	0.860826
-646.227385	6.282210	0.865830
-649.741799	-3.507393	0.870835
-653.791457	5.651228	0.875840
-657.120212	0.959786	0.880845
-660.432907	-3.397722	0.885850
-664.549008	-4.192478	0.890854
-668.040728	-3.121237	0.895859
-672.466426	7.703656	0.900864
-676.378580	-4.040543	0.905869
-680.140224	0.004574	0.910874
-683.865091	-4.656363	0.915878
-687.233053	-0.705246	0.920883
-691.033162	4.578364	0.925888
-695.088005	3.010944	0.930893
-698.862826	5.014544	0.935898
-702.537843	5.190101	0.940902
-706.003274	-7.812485	0.945907
-710.217576	5.068504	0.950912
-713.879532	-1.728704	0.955917
-717.800289	4.860407	0.960922
-721.550379	2.698381	0.965926
-724.906775	-2.071544	0.970931
-728.563252	-3.607835	0.975936
-732.158293	3.933075	0.980941
-736.186622	-2.172860	0.985946
-739.986338	7.710643	0.990950
-744.056192	-5.659060	0.995955
-747.765180	-4.794791	1.000960
-751.574507	1.556160	1.005965
-755.264481	6.704877	1.010970
-758.945589	0.775406	1.015974
-762.321880	-0.445025	1.020979
-766.012218	8.164557	1.025984
-769.925437	5.826903	1.030989
-773.817043	8.179402	1.035994
-777.858551	7.311560	1.040998
-781.399305	2.427281	1.046003
-785.163543	7.932953	1.051008
-789.166727	7.111435	1.056013
-792.708167	7.457548	1.061018
-796.405048	8.193474	1.066022
-800.218984	-0.373093	1.071027
-804.443786	-3.996868	1.076032
-807.894997	-10.144158	1.081037
-811.414316	-11.157249	1.086042
-815.565153	-6.898783	1.091046
-819.401127	2.338156	1.096051
-823.245015	3.942037	1.101056
-826.458974	-0.006002	1.106061
-830.206329	0.265363	1.111066
-834.311505	2.655362	1.116070
-837.595068	-0.031078	1.121075
-841.569125	1.224138	1.126080
-845.646623	-0.931705	1.131085
-849.168037	-0.105863	1.136090
-853.182174	-4.617526	1.141094
-856.629518	-4.254753	1.146099
-860.702753	1.073511	1.151104
-863.849423	3.329793	1.156109
-867.519326	7.966773	1.161114
-871.481856	3.676380	1.166118
-875.323565	-0.336744	1.171123
-879.398328	-5.378329	1.176128
-883.012851	-5.757698	1.181133
-886.952184	2.198847	1.186138
-890.736258	7.931020	1.191142
-894.341984	4.155672	1.196147
-898.057323	3.158932	1.201152
-901.955942	-2.249158	1.206157
-905.412534	-5.130823	1.211162
-909.507958	-6.731332	1.216166
-913.142123	-3.746379	1.221171
-917.070389	2.221734	1.226176
-920.667335	0.664338	1.231181
-924.370985	2.601837	1.236186
-928.141171	1.007876	1.241190
-931.677138	-6.902121	1.246195
-935.412712	1.100400	1.251200
-939.388423	-3.365280	1.256205
-943.156327	-4.712533	1.261210
-946.921664	7.059423	1.266214
-950.357575	-3.121510	1.271219
-954.494355	5.807996	1.276224
-958.134793	1.006506	1.281229
-962.004034	-4.413673	1.286234
-966.124001	-5.869003	1.291238
-969.380755	-3.499807	1.296243
-973.547558	-1.216326	1.301248
-976.916458	-6.696339	1.306253
-980.557702	-2.202338	1.311258
-984.297738	-4.550971	1.316262
-988.280612	-4.975556	1.321267
-992.280712	-5.898061	1.326272
-995.610532	-8.882330	1.331277
-999.857907	-13.087771	1.336282
-1003.874448	2.093798	1.341286
-1007.170656	-4.666071	1.346291
-1011.003843	0.062209	1.351296
-1014.541335	-0.614858	1.356301
-1018.403224	-4.980406	1.361306
-1022.528214	1.082357	1.366310
-1026.176511	-7.677409	1.371315
-1029.962976	3.641559	1.376320
-1033.376107	-4.051033	1.381325
-1036.991542	-4.307757	1.386330
-1041.084000	-0.681556	1.391334
-1044.598374	-5.805770	1.396339
-1048.762831	-4.195595	1.401344
-1052.522727	2.023966	1.406349
-1056.302334	2.278172	1.411354
-1059.965694	6.657230	1.416358
-1063.331547	5.288811	1.421363
-1067.132029	8.907138	1.426368
-1070.904652	1.632326	1.431373
-1074.442422	1.419532	1.436378
-1078.727301	3.344075	1.441382
-1082.605806	-1.562070	1.446387
-1086.269282	6.108085	1.451392
-1089.653862	2.431111	1.456397
-1093.579751	-9.198984	1.461402
-1097.569770	1.392810	1.466406
-1101.309598	-1.376905	1.471411
-1105.061548	2.579277	1.476416
-1108.817434	4.992444	1.481421
-1112.481297	3.954689	1.486426
-1116.160899	6.844988	1.491430
-1119.906761	4.316701	1.496435
-1124.044177	5.068163	1.501440
-1127.569651	-3.769436	1.506445
-1130.872293	2.347594	1.511450
-1134.864313	7.163250	1.516454
-1138.882906	-3.277423	1.521459
-1142.486709	-2.052356	1.526464
-1145.926740	-1.381551	1.531469
-1150.113753	4.583435	1.536474
-1154.010077	2.835299	1.541478
-1157.631049	1.000018	1.546483
-1161.797638	7.321874	1.551488
-1165.335389	0.191149	1.556493
-1168.678965	-4.938603	1.561498
-1172.732160	10.004287	1.566502
-1176.075017	0.197944	1.571507
-1180.148043	0.624218	1.576512
-1183.992400	-2.772419	1.581517
-1187.930475	0.179300	1.586522
-1191.574914	-1.214193	1.591526
-1195.105600	-6.624791	1.596531
-1198.964312	10.672293	1.601536
-1202.611492	-5.591242	1.606541
-1206.245688	-2.612359	1.611546
-1210.230519	0.773691	1.616550
-1213.911931	-5.846038	1.621555
-1218.155899	0.345089	1.626560
-1221.772112	-0.190399	1.631565
-1225.422972	-6.287248	1.636570
-1229.388755	1.372571	1.641574
-1232.573933	-6.831058	1.646579
-1236.398290	0.122822	1.651584
-1240.245473	-7.794225	1.656589
-1244.459735	-8.065154	1.661594
-1247.979392	-5.245632	1.666598
-1251.509683	-5.271683	1.671603
-1255.643510	4.941949	1.676608
-1258.955320	-0.696828	1.681613
-1262.760143	-0.470867	1.686618
-1266.725513	12.070235	1.691622
-1270.474637	-3.487751	1.696627
-1274.473761	6.131230	1.701632
-1278.131205	5.124094	1.706637
-1281.897290	3.269244	1.711642
-1285.442839	0.779331	1.716646
-1288.800306	1.042156	1.721651
-1292.687136	-1.175993	1.726656
-1296.803797	-4.586932	1.731661
-1300.782466	-4.643683	1.736666
-1304.559241	-1.264075	1.741670
-1308.372195	-5.216994	1.746675
-1311.936736	1.607463	1.751680
-1315.223358	2.439935	1.756685
-1318.827370	2.570276	1.761690
-1322.910642	1.045054	1.766694
-1326.930847	-6.915998	1.771699
-1331.093245	-5.799283	1.776704
-1334.520859	-4.575504	1.781709
-1338.005895	-5.196181	1.786714
-1341.969489	-1.149766	1.791718
-1345.426482	-6.848785	1.796723
-1349.372970	3.957566	1.801728
-1353.189623	-3.914091	1.806733
-1357.023398	-5.721326	1.811738
-1360.862920	-1.223350	1.816742
-1364.413083	-7.135672	1.821747
-1368.415498	0.484379	1.826752
-1371.926439	7.817136	1.831757
-1375.204692	-3.779844	1.836762
-1379.436076	1.780115	1.841766
-1383.250353	-4.807157	1.846771
-1387.086438	1.140001	1.851776
-1390.769024	-4.936245	1.856781
-1394.486604	-9.949061	1.861786
-1398.540584	-1.203509	1.866790
-1402.094407	-2.540151	1.871795
-1406.035540	-7.606915	1.876800
-1409.276456	4.663019	1.881805
-1413.069738	-3.453759	1.886810
-1417.118487	3.468170	1.891814
-1421.217424	-2.959648	1.896819
-1425.034168	-1.142019	1.901824
-1428.230956	-0.541583	1.906829
-1432.083041	-3.349730	1.911834
-1435.943326	12.439634	1.916838
-1439.307759	-1.554128	1.921843
-1443.622361	-3.258551	1.926848
-1447.419756	2.428613	1.931853
-1450.931082	-4.841374	1.936858
-1454.946588	-1.136831	1.941862
-1458.357255	-0.670142	1.946867
-1462.254661	-1.974940	1.951872
-1466.186809	2.837437	1.956877
-1469.458398	-10.561236	1.961882
-1473.701992	-1.498856	1.966886
-1477.238558	1.137062	1.971891
-1481.351495	-4.620842	1.976896
-1484.886408	3.381194	1.981901
-1488.184684	-0.112521	1.986906
-1492.491617	6.317430	1.991910
-1495.905532	-2.010087	1.996915
-1500.266347	0.787144	2.006912
-1501.132387	2.293393	2.016909
-1498.367667	1.717935	2.026906
-1495.675254	-2.683767	2.036902
-1493.666730	-1.462707	2.046899
-1491.433281	-3.487018	2.056896
-1489.639363	-4.373887	2.066893
-1487.867280	-2.338779	2.076890
-1486.055952	-3.164615	2.086886
-1483.775574	-5.576384	2.096883
-1482.176675	-3.570012	2.106880
-1480.112426	0.560102	2.116877
-1478.050611	-0.482656	2.126874
-1476.072115	-9.691139	2.136870
-1474.672456	-5.095903	2.146867
-1472.822274	-0.361489	2.156864
-1470.878486	-4.244886	2.166861
-1468.747152	-6.818767	2.176858
-1467.231818	-4.479494	2.186854
-1465.138823	-1.339172	2.196851
-1463.393670	3.446094	2.206848
-1460.827956	1.174226	2.216845
-1459.137303	-0.717297	2.226842
-1457.574773	1.137645	2.236838
-1455.882311	1.961297	2.246835
-1453.839894	4.393800	2.256832
-1452.067140	5.055061	2.266829
-1450.238909	4.341343	2.276826
-1447.966556	6.588515	2.286822
-1446.049543	7.170063	2.296819
-1444.662592	4.711424	2.306816
-1442.584515	4.511639	2.316813
-1440.465630	-1.524893	2.326810
-1438.434690	-2.388830	2.336806
-1436.802544	5.559755	2.346803
-1435.054417	7.576476	2.356800
-1433.020215	5.370244	2.366797
-1431.361929	-3.312128	2.376794
-1429.253784	0.468616	2.386790
-1427.509080	2.071353	2.396787
-1425.587596	1.968429	2.406784
-1423.485138	-2.051680	2.416781
-1421.422045	-6.161455	2.426778
-1420.056780	-0.878551	2.436774
-1417.937500	0.245268	2.446771
-1415.996142	-0.863317	2.456768
-1414.263856	-1.531687	2.466765
-1412.590937	0.337507	2.476762
-1410.328883	2.776171	2.486758
-1408.707741	3.982406	2.496755
-1406.937476	11.390347	2.506752
-1404.905687	1.610345	2.516749
-1402.806515	1.704153	2.526746
-1401.061640	3.162621	2.536742
-1399.078491	4.229213	2.546739
-1397.433176	2.687358	2.556736
-1395.422527	4.129419	2.566733
-1393.381791	0.092262	2.576730
-1391.748919	0.001781	2.586726
-1389.710219	4.524430	2.596723
-1387.884483	3.570880	2.606720
-1386.149768	4.766704	2.616717
-1384.236081	3.227760	2.626714
-1382.380046	6.390257	2.636710
-1380.304150	3.075437	2.646707
-1378.048165	-0.190484	2.656704
-1376.748837	4.418076	2.666701
-1374.918606	-2.170748	2.676698
-1373.194290	-1.229623	2.686694
-1371.188340	2.700313	2.696691
-1368.888358	-3.107641	2.706688
-1367.193208	-3.994882	2.716685
-1365.595864	-2.970687	2.726682
-1363.432582	0.628311	2.736678
-1361.749293	1.577278	2.746675
-1359.886276	3.774274	2.756672
-1357.901437	6.543160	2.766669
-1356.029447	-0.969717	2.776666
-1354.209435	4.142623	2.786662
-1352.012853	-0.494340	2.796659
-1350.333768	-2.539151	2.806656
-1348.467862	5.023119	2.816653
-1346.714901	0.524802	2.826650
-1344.696975	2.392860	2.836646
-1342.720703	6.653168	2.846643
-1340.682949	4.004128	2.856640
-1339.338269	5.563375	2.866637
-1337.278996	3.139468	2.876634
-1335.590767	0.512527	2.886630
-1333.411066	-0.116073	2.896627
-1331.857917	0.932721	2.906624
-1329.776688	-1.211983	2.916621
-1327.829643	-1.065133	2.926618
-1325.766730	3.304397	2.936614
-1324.057638	3.608313	2.946611
-1322.158665	2.886451	2.956608
-1320.208706	3.209068	2.966605
-1318.488880	-0.889918	2.976602
-1316.452622	-6.222559	2.986598
-1314.627321	-3.677209	2.996595
-1312.716595	-0.403930	3.006592
-1310.993086	1.489817	3.016589
-1309.429534	-0.490477	3.026586
-1306.709614	-4.901532	3.036582
-1305.556901	-2.866272	3.046579
-1303.325138	-3.176170	3.056576
-1301.623333	1.844258	3.066573
-1300.059521	-1.348186	3.076570
-1297.946032	-5.617928	3.086566
-1295.784639	-3.832583	3.096563
-1294.310263	-0.937260	3.106560
-1292.120264	-11.556937	3.116557
-1290.061610	-7.683043	3.126554
-1288.036249	2.126305	3.136550
-1286.364827	-1.308307	3.146547
-1285.013885	-4.417155	3.156544
-1282.920952	0.796943	3.166541
-1280.907078	-2.403237	3.176538
-1278.952221	-3.022437	3.186534
-1277.272691	-0.780452	3.196531
-1275.292211	-1.649477	3.206528
-1273.496687	1.524254	3.216525
-1271.365969	3.178534	3.226522
-1269.677635	1.111218	3.236518
-1267.864877	-1.364773	3.246515
-1265.698835	3.527724	3.256512
-1263.993485	-1.634638	3.266509
-1262.274799	-1.834262	3.276506
-1260.372089	-15.401067	3.286502
-1258.586746	-3.234947	3.296499
-1256.954523	-5.063003	3.306496
-1254.358102	7.424643	3.316493
-1252.428075	-3.785873	3.326490
-1250.647874	-5.340958	3.336486
-1248.971912	-8.069698	3.346483
-1247.271743	-8.619454	3.356480
-1245.126919	-9.675960	3.366477
-1243.302438	-1.491180	3.376474
-1241.361967	0.954989	3.386470
-1239.603038	-2.563797	3.396467
-1237.860961	1.973516	3.406464
-1236.093248	1.438249	3.416461
-1233.877456	-0.922383	3.426458
-1232.250861	-1.169018	3.436454
-1230.052221	-3.565432	3.446451
-1228.274758	2.899178	3.456448
-1226.498754	4.921479	3.466445
-1224.653369	3.078562	3.476442
-1222.709935	-0.220550	3.486438
-1220.789401	6.381136	3.496435
-1218.838780	-0.734177	3.506432
-1217.275506	3.185313	3.516429
-1215.220483	3.491121	3.526426
-1213.217929	1.836212	3.536422
-1211.586812	3.327736	3.546419
-1209.722350	3.397530	3.556416
-1207.659673	1.801460	3.566413
-1206.012177	-2.337231	3.576410
-1203.990856	-3.283980	3.586406
-1201.632274	4.077567	3.596403
-1200.344001	6.246083	3.606400
-1198.310490	-0.965661	3.616397
-1196.532031	7.381975	3.626394
-1194.616828	1.515691	3.636390
-1192.564858	4.012293	3.646387
-1190.673038	-0.741802	3.656384
-1188.820574	4.179692	3.666381
-1187.198428	3.393586	3.676378
-1185.226277	5.657683	3.686374
-1183.256497	0.404884	3.696371
-1181.452512	-1.653409	3.706368
-1179.380597	2.399671	3.716365
-1177.851706	3.583109	3.726362
-1175.775450	-1.420809	3.736358
-1174.085696	3.820696	3.746355
-1172.101979	9.180081	3.756352
-1170.026546	6.490265	3.766349
-1168.291341	1.231119	3.776346
-1166.578621	4.593804	3.786342
-1164.419222	-1.334163	3.796339
-1162.325653	5.902584	3.806336
-1161.106408	8.358033	3.816333
-1159.001394	7.236873	3.826330
-1156.923265	2.625085	3.836326
-1155.134915	4.631465	3.846323
-1152.991869	5.556502	3.856320
-1151.491020	5.334258	3.866317
-1149.440554	6.153866	3.876314
-1147.558178	7.547335	3.886310
-1145.941383	12.623143	3.896307
-1143.731516	13.129644	3.906304
-1142.182555	10.844834	3.916301
-1140.065015	13.406876	3.926298
-1138.093445	9.451264	3.936294
-1136.184544	4.295488	3.946291
-1134.738245	9.241702	3.956288
-1132.854685	8.777878	3.966285
-1130.878281	9.413793	3.976282
-1128.742920	11.315939	3.986278
-1126.768732	13.472219	3.996275
-1125.302608	8.256130	4.006272
-1123.500849	9.582435	4.016269
-1121.478352	6.487945	4.026266
-1119.513070	5.706967	4.036262
-1117.216758	0.963276	4.046259
-1115.761894	2.425822	4.056256
-1114.084725	7.289323	4.066253
-1112.023619	3.528600	4.076250
-1110.136735	3.202539	4.086246
-1108.581233	8.053341	4.096243
-1106.069685	11.597821	4.106240
-1104.549390	-0.234307	4.116237
-1102.668067	4.172848	4.126234
-1100.521005	4.513100	4.136230
-1098.718304	1.002660	4.146227
-1097.061479	5.098209	4.156224
-1095.332386	3.578046	4.166221
-1093.203258	-1.577191	4.176218
-1091.481171	-2.614386	4.186214
-1089.240604	-0.039457	4.196211
-1087.683225	-3.467061	4.206208
-1085.670625	1.775168	4.216205
-1083.889298	-3.514393	4.226202
-1081.979057	2.680483	4.236198
-1080.000782	4.915915	4.246195
-1078.429596	-0.182244	4.256192
-1076.206550	2.764434	4.266189
-1074.137134	8.481445	4.276186
-1072.498458	3.490261	4.286182
-1070.438750	-1.183140	4.296179
-1068.786387	6.280782	4.306176
-1067.416966	5.300592	4.316173
-1065.195435	0.252808	4.326170
-1063.287331	-0.181212	4.336166
-1061.089093	0.195328	4.346163
-1059.168881	1.882306	4.356160
-1057.796533	-2.137558	4.366157
-1056.009309	1.622216	4.376154
-1054.084127	-4.768589	4.386150
-1051.807680	-9.258666	4.396147
-1049.973309	-10.231735	4.406144
-1048.284887	-2.276427	4.416141
-1046.434455	-4.898702	4.426138
-1044.601744	-1.034098	4.436134
-1042.729755	-3.112706	4.446131
-1040.424100	-3.496805	4.456128
-1038.652709	-3.824347	4.466125
-1036.915035	-3.070729	4.476122
-1034.890896	-8.631578	4.486118
-1033.436795	-0.764474	4.496115
-1031.524358	-0.193411	4.506112
-1029.684572	4.995130	4.516109
-1027.407383	-0.745513	4.526106
-1025.809033	1.249282	4.536102
-1023.540191	4.094066	4.546099
-1022.081362	6.543994	4.556096
-1019.917537	11.130725	4.566093
-1018.119304	2.024491	4.576090
-1016.188832	0.082477	4.586086
-1014.370979	-0.761273	4.596083
-1012.480518	-0.025578	4.606080
-1010.405168	-1.762450	4.616077
-1008.754143	-6.333644	4.626074
-1007.051331	-3.919278	4.636070
-1005.076064	-4.684530	4.646067
-1003.151818	3.356387	4.656064
-1001.348771	3.170049	4.666061
-999.550957	6.798403	4.676058
-997.642732	0.959082	4.686054
-995.411297	-2.684602	4.696051
-993.959614	10.970813	4.706048
-992.079218	3.720622	4.716045
-989.902185	3.558214	4.726042
-988.004330	8.819012	4.736038
-986.263506	1.464738	4.746035
-984.468549	4.571119	4.756032
-982.229599	6.388766	4.766029
-980.850013	7.356042	4.776026
-979.200705	3.601657	4.786022
-976.682394	9.144038	4.796019
-975.028122	7.179112	4.806016
-973.043638	7.376609	4.816013
-971.363238	4.136988	4.826010
-969.418067	0.519934	4.836006
-967.358480	5.315476	4.846003
-965.626575	4.471483	4.856000
-963.823384	7.240135	4.865997
-961.814690	2.207991	4.875994
-960.189107	8.224951	4.885990
-957.590854	4.043660	4.895987
-956.341643	2.620953	4.905984
-954.749843	4.426014	4.915981
-952.675075	11.049580	4.925978
-950.607223	5.233459	4.935974
-948.607291	0.328108	4.945971
-946.459760	5.874878	4.955968
-945.082664	6.923612	4.965965
-943.073122	9.880539	4.975962
-941.240637	3.077278	4.985958
-939.396849	11.066440	4.995955
-937.466409	8.018661	5.005952
-935.598803	1.988336	5.015949
-933.691622	11.287416	5.025946
-931.968363	6.857976	5.035942
-929.957891	10.880242	5.045939
-928.334787	7.416901	5.055936
-925.936654	12.531381	5.065933
-924.416935	10.141006	5.075930
-922.709161	1.575173	5.085926
-920.506275	-3.841237	5.095923
-918.769230	7.406205	5.105920
-916.884254	4.718769	5.115917
-914.603130	10.045020	5.125914
-912.970687	1.909861	5.135910
-911.298714	-0.713737	5.145907
-909.313011	0.712295	5.155904
-907.373016	4.769196	5.165901
-905.742254	-1.031548	5.175898
-903.510374	-2.511875	5.185894
-902.027765	0.284567	5.195891
-900.143661	4.949417	5.205888
-898.170252	4.472247	5.215885
-896.394429	2.617695	5.225882
-894.079824	0.705828	5.235878
-892.310973	-2.322096	5.245875
-890.558928	0.684196	5.255872
-888.831504	0.513258	5.265869
-886.889832	-1.115244	5.275866
-884.693847	3.051067	5.285862
-882.794145	-2.859465	5.295859
-881.104731	0.453991	5.305856
-879.553200	0.251597	5.315853
-877.586652	-0.303427	5.325850
-875.655720	-4.281592	5.335846
-873.687296	2.599372	5.345843
-871.542266	-1.259829	5.355840
-869.855752	-3.268982	5.365837
-868.088541	-2.782785	5.375834
-865.901860	-0.091379	5.385830
-864.374160	0.297609	5.395827
-862.430151	-2.842179	5.405824
-860.684924	4.274316	5.415821
-859.007306	9.530696	5.425818
-856.829160	1.088072	5.435814
-854.807552	4.936546	5.445811
-852.906445	0.606632	5.455808
-851.129495	-2.540045	5.465805
-849.605848	3.878211	5.475802
-847.578071	0.427245	5.485798
-845.470401	-1.832827	5.495795
-843.444617	-2.186566	5.505792
-841.789400	1.539055	5.515789
-839.771960	-2.057942	5.525786
-837.985781	1.127473	5.535782
-836.122473	-2.756074	5.545779
-834.449574	-0.821030	5.555776
-832.446288	-1.025464	5.565773
-830.467177	0.015219	5.575770
-828.570152	-1.856554	5.585766
-826.936449	-2.005057	5.595763
-824.633450	1.416123	5.605760
-823.128084	-2.390566	5.615757
-821.280226	7.815098	5.625754
-819.380602	0.249848	5.635750
-817.318689	-1.388592	5.645747
-815.514482	5.165296	5.655744
-813.691863	3.637488	5.665741
-811.961245	3.030904	5.675738
-809.898668	-0.429971	5.685734
-807.693929	-4.470123	5.695731
-805.931335	-1.089759	5.705728
-804.223851	6.670326	5.715725
-802.448582	5.902344	5.725722
-800.813299	4.068789	5.735718
-798.511678	4.382271	5.745715
-796.722742	1.829932	5.755712
-795.021101	3.904312	5.765709
-792.973847	2.594450	5.775706
-791.029900	1.452500	5.785702
-788.852280	2.815218	5.795699
-787.202219	-3.652758	5.805696
-785.555699	-2.814228	5.815693
-783.853566	-0.672743	5.825690
-781.991495	0.472231	5.835686
-779.746615	0.969750	5.845683
-777.736200	-0.418358	5.855680
-776.133067	-1.371780	5.865677
-774.398496	0.606452	5.875674
-772.107037	-1.004178	5.885670
-770.379571	2.225728	5.895667
-768.942760	4.397740	5.905664
-766.976510	6.598634	5.915661
-764.454851	4.307462	5.925658
-763.058311	5.643005	5.935654
-761.260965	4.651907	5.945651
-759.460576	2.272301	5.955648
-757.342019	4.682605	5.965645
-755.264566	5.246418	5.975642
-753.358950	2.831760	5.985638
-751.870225	-1.600835	5.995635
-749.894548	5.458774	6.005632
-748.153945	4.458845	6.015629
-745.774092	0.361792	6.025626
-743.933768	1.898614	6.035622
-742.665223	1.399422	6.045619
-740.442514	-0.422689	6.055616
-738.745770	1.644650	6.065613
-736.943602	6.197175	6.075610
-734.736055	0.962240	6.085606
-732.645432	2.752520	6.095603
-730.970201	-0.139527	6.105600
-729.314661	1.923822	6.115597
-727.660835	0.542396	6.125594
-725.212848	-1.297424	6.135590
-723.592049	0.486941	6.145587
-721.626058	3.892904	6.155584
-719.628344	1.418190	6.165581
-717.711498	1.764553	6.175578
-716.232254	0.683814	6.185574
-714.462578	5.660455	6.195571
-712.316875	3.253222	6.205568
-710.464209	-2.491088	6.215565
-708.458138	-6.888754	6.225562
-706.461509	0.503605	6.235558
-704.714114	0.437602	6.245555
-702.924661	1.501408	6.255552
-701.170426	6.455807	6.265549
-699.266795	6.070536	6.275546
-697.254226	3.209135	6.285542
-695.538068	7.186782	6.295539
-693.472625	3.800951	6.305536
-691.691018	8.632490	6.315533
-689.958944	2.633417	6.325530
-688.062977	2.554965	6.335526
-685.806897	0.457619	6.345523
-684.081875	1.083134	6.355520
-682.232878	0.093480	6.365517
-680.546184	1.678827	6.375514
-678.416304	-1.963086	6.385510
-676.651448	-0.892677	6.395507
-674.943679	-5.282215	6.405504
-672.825901	6.324871	6.415501
-670.855916	1.075008	6.425498
-669.293379	-0.053207	6.435494
-667.283551	-5.241927	6.445491
-665.383449	-3.528393	6.455488
-663.737175	4.297196	6.465485
-661.375791	0.619119	6.475482
-659.669364	-2.459659	6.485478
-658.038647	-2.919804	6.495475
-656.120681	-6.711091	6.505472
-654.006320	-6.174510	6.515469
-652.180261	-0.974342	6.525466
-650.205775	2.656655	6.535462
-648.632331	-0.329740	6.545459
-646.904870	-3.776114	6.555456
-644.496216	3.064601	6.565453
-642.889791	1.619016	6.575450
-640.903305	1.930144	6.585446
-639.333442	3.863189	6.595443
-637.155469	3.222193	6.605440
-635.313891	-1.714347	6.615437
-633.574424	-0.460136	6.625434
-631.783182	3.200339	6.635430
-629.764449	-5.532189	6.645427
-627.867560	2.014073	6.655424
-625.844668	-2.406603	6.665421
-623.788399	-5.604287	6.675418
-622.314794	-6.147328	6.685414
-620.472994	-5.102350	6.695411
-618.535923	-3.002692	6.705408
-616.587722	-3.994720	6.715405
-614.820371	2.912587	6.725402
-612.694927	3.423574	6.735398
-611.180497	1.561028	6.745395
-609.256282	5.089617	6.755392
-607.005103	6.914457	6.765389
-605.467847	8.569348	6.775386
-603.362353	3.380834	6.785382
-601.631802	5.865307	6.795379
-599.733118	4.146687	6.805376
-597.625502	8.315279	6.815373
-596.009118	3.327680	6.825370
-594.375066	9.300270	6.835366
-592.108931	4.106328	6.845363
-590.099510	7.966513	6.855360
-588.483857	8.669720	6.865357
-586.650241	5.742641	6.875354
-584.676621	12.816922	6.885350
-582.919644	8.789282	6.895347
-580.897493	9.188775	6.905344
-579.540915	9.166564	6.915341
-577.007200	10.152119	6.925338
-574.922652	8.158164	6.935334
-573.499820	8.494112	6.945331
-571.570902	10.986454	6.955328
-569.917659	8.696984	6.965325
-567.837008	12.422048	6.975322
-565.578741	6.907367	6.985318
-563.963394	9.071346	6.995315
-562.673623	11.720392	7.005312
-560.122760	11.720908	7.015309
-558.216709	11.057446	7.025306
-556.490652	4.757111	7.035302
-554.879833	7.522989	7.045299
-553.085882	9.314071	7.055296
-551.133047	6.289879	7.065293
-548.911548	2.806196	7.075290
-547.233178	6.253691	7.085286
-545.427837	8.493366	7.095283
-543.358997	13.312444	7.105280
-541.554222	6.563081	7.115277
-539.613127	12.897593	7.125274
-537.923070	9.008315	7.135270
-535.659176	5.167600	7.145267
-534.097933	9.508620	7.155264
-532.227724	6.698986	7.165261
-530.323432	6.943249	7.175258
-528.366176	3.054765	7.185254
-526.659026	8.281326	7.195251
-524.546269	4.774024	7.205248
-522.584390	5.490966	7.215245
-520.902629	11.553812	7.225242
-519.164173	6.866204	7.235238
-517.370774	3.360346	7.245235
-515.251303	3.282351	7.255232
-513.381246	4.858043	7.265229
-511.660677	8.847660	7.275226
-509.646543	4.789759	7.285222
-507.769165	2.720325	7.295219
-505.794461	6.042299	7.305216
-503.877436	5.032747	7.315213
-502.304419	8.927145	7.325210
-499.996820	8.013015	7.335206
-498.318598	0.276400	7.345203
-496.849498	9.507021	7.355200
-494.771805	1.820829	7.365197
-492.781676	-1.689527	7.375194
-490.643003	8.616997	7.385190
-489.077781	2.128887	7.395187
-487.014949	6.871562	7.405184
-485.214323	6.362963	7.415181
-483.395434	10.187520	7.425178
-481.515367	8.323542	7.435174
-479.498795	5.594734	7.445171
-477.878384	11.253150	7.455168
-475.942887	11.516982	7.465165
-474.277602	7.115431	7.475162
-472.030339	7.064144	7.485158
-470.164496	7.117423	7.495155
-468.019893	3.760792	7.505152
-466.394413	9.261442	7.515149
-464.677514	5.789674	7.525146
-462.923131	6.311437	7.535142
-460.797837	6.764427	7.545139
-459.225254	14.166838	7.555136
-457.065551	13.404968	7.565133
-455.097857	14.499558	7.575130
-453.404906	5.909531	7.585126
-451.281965	3.073959	7.595123
-449.636310	7.036539	7.605120
-447.760265	5.440034	7.615117
-446.067145	6.939797	7.625114
-443.945713	5.572313	7.635110
-442.073597	6.186521	7.645107
-440.196370	9.003964	7.655104
-438.336477	12.847986	7.665101
-436.437296	8.053395	7.675098
-434.515153	4.321944	7.685094
-432.505120	3.716183	7.695091
-430.655187	1.348755	7.705088
-428.887908	2.379726	7.715085
-427.033100	3.562067	7.725082
-425.536661	7.500459	7.735078
-423.267479	6.250308	7.745075
-421.190280	12.198724	7.755072
-419.814777	8.804509	7.765069
-417.923697	8.281210	7.775066
-415.813186	10.559883	7.785062
-413.987536	8.795376	7.795059
-412.281838	4.226852	7.805056
-410.382838	-1.130876	7.815053
-408.324821	7.250612	7.825050
-406.397508	5.446931	7.835046
-404.345485	10.186762	7.845043
-402.521988	8.033738	7.855040
-400.867285	3.166490	7.865037
-399.172991	0.081586	7.875034
-397.048599	6.637660	7.885030
-395.026340	4.179425	7.895027
-393.373811	4.956608	7.905024
-391.453650	6.569998	7.915021
-389.589398	8.782639	7.925018
-387.561085	4.005041	7.935014
-385.905425	10.068077	7.945011
-384.078857	9.000583	7.955008
-382.080172	7.620590	7.965005
-379.923677	7.456476	7.975002
-378.364125	4.389950	7.984998
-376.535351	12.263412	7.994995
-374.385369	12.155353	8.004992
-372.729867	10.653622	8.014989
-370.804322	12.783829	8.024986
-368.971681	5.321123	8.034982
-366.758235	7.434352	8.044979
-365.274495	8.705667	8.054976
-363.548515	13.829478	8.064973
-361.357596	9.223184	8.074970
-359.472462	3.978512	8.084966
-357.553959	4.527493	8.094963
-356.021054	9.188037	8.104960
-353.947832	11.215852	8.114957
-351.815885	15.027870	8.124954
-350.034304	14.197331	8.134950
-348.183970	15.469397	8.144947
-346.442076	10.506584	8.154944
-344.518769	12.320620	8.164941
-342.573737	3.013148	8.174938
-340.722074	11.036044	8.184934
-339.021209	11.706548	8.194931
-337.262836	9.441413	8.204928
-335.121534	11.718402	8.214925
-333.349778	10.037471	8.224922
-331.467994	5.221005	8.234918
-329.403282	8.116603	8.244915
-327.545934	4.863847	8.254912
-325.818696	7.384179	8.264909
-323.839883	7.387314	8.274906
-322.160966	9.564986	8.284902
-320.083403	6.283944	8.294899
-318.164557	3.786570	8.304896
-316.389646	9.437523	8.314893
-314.449202	6.608812	8.324890
-312.624489	4.718037	8.334886
-310.819980	4.822610	8.344883
-308.932370	4.680149	8.354880
-306.925710	0.720441	8.364877
-304.883671	0.490629	8.374874
-303.330687	2.020019	8.384870
-301.453225	4.094479	8.394867
-299.222308	4.920298	8.404864
-297.610460	10.332065	8.414861
-296.016572	13.369697	8.424858
-293.861444	9.411795	8.434854
-291.698193	4.713056	8.444851
-290.029856	4.514943	8.454848
-288.513492	7.793122	8.464845
-286.512450	-0.094049	8.474842
-284.386488	4.147045	8.484838
-282.813479	6.832173	8.494835
-280.444281	3.884485	8.504832
-278.851144	10.224272	8.514829
-276.862523	6.282292	8.524826
-274.906053	3.706157	8.534822
-273.413950	4.410122	8.544819
-271.423220	8.093453	8.554816
-269.593732	7.351556	8.564813
-267.683798	9.777737	8.574810
-265.655532	6.317447	8.584807
-263.837896	2.816614	8.594803
-261.847627	4.007408	8.604800
-260.122891	3.967599	8.614797
-258.120189	-0.165701	8.624794
-256.248012	2.028250	8.634791
-254.731470	8.697356	8.644787
-252.528826	3.339377	8.654784
-250.565817	2.967825	8.664781
-248.872262	6.798175	8.674778
-247.125996	3.636036	8.684775
-244.840431	-0.886843	8.694771
-243.218545	-1.897043	8.704768
-241.251179	3.779821	8.714765
-239.492631	9.025358	8.724762
-237.766002	6.300932	8.734759
-235.670225	0.040835	8.744755
-233.775718	11.527610	8.754752
-232.088306	5.545435	8.764749
-229.778688	-0.049829	8.774746
-227.640862	1.380862	8.784743
-226.101224	-5.581784	8.794739
-224.802408	-1.995154	8.804736
-222.487918	-4.414116	8.814733
-220.852014	-7.605927	8.824730
-218.728042	1.695082	8.834727
-217.077236	-4.804071	8.844723
-214.841388	-8.329580	8.854720
-213.266560	-2.941865	8.864717
-211.489390	4.472591	8.874714
-209.151808	-4.797821	8.884711
-207.451394	-8.012547	8.894707
-205.623400	2.718532	8.904704
-203.854471	2.722543	8.914701
-201.861213	-4.517084	8.924698
-200.189301	-8.478223	8.934695
-198.419427	-1.813816	8.944691
-196.307899	-7.183805	8.954688
-194.484636	1.127004	8.964685
-192.840816	-4.202688	8.974682
-190.386278	-8.034439	8.984679
-188.629050	-6.559007	8.994675
-187.014869	-2.771536	9.004672
-185.228857	0.630377	9.014669
-183.044424	-6.525836	9.024666
-181.155607	1.177753	9.034663
-179.368471	5.211822	9.044659
-177.203450	0.033038	9.054656
-175.469787	2.342075	9.064653
-173.882784	2.648810	9.074650
-172.490797	-0.424482	9.084647
-169.763943	-0.920279	9.094643
-168.028331	0.312650	9.104640
-166.455945	-6.760723	9.114637
-164.581301	-3.893709	9.124634
-162.638874	-7.588614	9.134631
-160.771101	-3.697208	9.144627
-158.736091	-3.116348	9.154624
-156.655831	-0.095680	9.164621
-154.997580	4.176685	9.174618
-153.105201	-0.413491	9.184615
-151.280736	0.370261	9.194611
-149.424832	0.005659	9.204608
-147.792177	3.918819	9.214605
-145.661106	-1.280609	9.224602
-144.071907	2.045996	9.234599
-141.846496	-0.878941	9.244595
-139.717004	0.751621	9.254592
-138.410092	-0.202156	9.264589
-136.248314	7.206058	9.274586
-134.176051	0.970980	9.284583
-132.601378	-5.413126	9.294579
-130.494351	1.271748	9.304576
-128.469128	7.135565	9.314573
-127.222658	5.447175	9.324570
-124.605580	3.343523	9.334567
-122.820402	3.871997	9.344563
-121.463503	4.442298	9.354560
-119.644532	2.205978	9.364557
-117.633169	3.947708	9.374554
-115.878168	4.484916	9.384551
-113.601926	7.934402	9.394547
-111.662266	4.182683	9.404544
-110.266867	9.363689	9.414541
-108.046090	3.548955	9.424538
-106.127572	-4.768615	9.434535
-104.379600	-1.894870	9.444531
-102.772024	0.929442	9.454528
-100.438150	5.294250	9.464525
-98.430138	4.764865	9.474522
-96.933549	1.651918	9.484519
-95.055435	1.379568	9.494515
-92.911008	6.422254	9.504512
-91.195766	5.087830	9.514509
-89.274678	-0.750595	9.524506
-87.814746	5.165519	9.534503
-85.378753	2.709188	9.544499
-84.008362	-2.932440	9.554496
-82.011791	5.511143	9.564493
-80.034535	5.753757	9.574490
-77.857217	2.114643	9.584487
-76.210544	4.895901	9.594483
-74.574902	2.778773	9.604480
-72.501927	3.643251	9.614477
-70.356957	4.606440	9.624474
-68.257539	6.353250	9.634471
-67.034039	10.161129	9.644467
-65.270443	4.390029	9.654464
-63.142578	4.480356	9.664461
-61.345178	4.930877	9.674458
-59.210340	4.306646	9.684455
-57.334717	3.947396	9.694451
-55.603259	9.194104	9.704448
-53.925837	6.101540	9.714445
-52.075974	0.138201	9.724442
-49.732913	3.011894	9.734439
-47.847755	0.863452	9.744435
-46.107455	1.674721	9.754432
-44.494104	-0.214882	9.764429
-42.221951	1.731941	9.774426
-40.509984	8.850578	9.784423
-38.824064	1.280347	9.794419
-36.811677	-5.746713	9.804416
-35.200091	2.382708	9.814413
-33.384307	3.154560	9.824410
-30.744048	1.601869	9.834407
-29.250749	-1.402994	9.844403
-27.503528	-0.852561	9.854400
-25.599878	2.053806	9.864397
-23.583171	-2.949300	9.874394
-21.906468	0.009815	9.884391
-19.838497	5.894022	9.894387
-18.181689	5.865952	9.904384
-16.124085	10.852824	9.914381
-14.223813	2.235278	9.924378
-12.506760	2.392908	9.934375
-10.587147	2.366414	9.944371
-8.821239	2.947244	9.954368
-6.756312	4.384219	9.964365
-4.932760	4.263143	9.974362
-3.452759	27.677217	9.984359
-2.234306	55.546007	9.994355
-0.944925	102.142750	10.004352
0.000000	149.121637	10.009357
0.600905	174.561729	10.014362
1.101970	208.443398	10.019367
1.747393	232.572995	10.024371
2.648462	257.842159	10.029376
2.183658	280.198868	10.034381
2.976358	289.359301	10.039386
3.123887	307.577042	10.044391
3.090324	314.341518	10.049395
3.496744	314.850843	10.054400
3.048170	326.704538	10.059405
3.031098	319.371971	10.064410
3.282292	329.444711	10.069415
3.389047	344.428056	10.074419
4.305303	353.106309	10.079424
4.031446	355.166292	10.084429
4.183694	333.567555	10.089434
3.871753	333.922170	10.094439
3.266121	338.738915	10.099443
3.794419	329.449365	10.104448
3.639464	348.157945	10.109453
4.220981	352.233932	10.114458
4.003727	367.333246	10.119463
4.206782	366.596182	10.124467
4.582999	370.916181	10.129472
3.939409	360.861666	10.134477
4.209170	345.046328	10.139482
4.342766	352.350950	10.144487
4.233347	359.392123	10.149491
4.472054	358.121996	10.154496
4.580353	364.523105	10.159501
4.129267	357.279146	10.164506
4.305149	368.250180	10.169511
4.375237	385.146743	10.174515
4.580781	384.962648	10.179520
4.488473	395.223006	10.184525
4.558475	389.030429	10.189530
4.598453	391.977620	10.194535
4.369250	389.792627	10.199539
4.459298	390.057397	10.204544
4.725409	400.111046	10.209549
4.528347	393.102978	10.214554
4.464346	396.503769	10.219559
4.764597	412.797632	10.224563
5.258737	421.161474	10.229568
4.856308	437.234016	10.234573
5.038675	436.136956	10.239578
5.326438	440.288991	10.244583
5.278034	443.437654	10.249587
5.567894	424.394309	10.254592
5.653717	425.618187	10.259597
5.358834	419.338956	10.264602
5.088019	411.341723	10.269607
5.073405	423.343707	10.274611
5.485855	429.295209	10.279616
5.610546	440.645320	10.284621
5.484598	428.052363	10.289626
5.363232	421.807719	10.294631
5.793879	442.945775	10.299635
6.113036	442.288664	10.304640
5.473224	429.383171	10.309645
5.718514	423.746686	10.314650
5.722663	434.541957	10.319655
5.889444	449.695499	10.324659
6.062500	448.456357	10.329664
5.648625	449.521977	10.334669
6.244123	451.961445	10.339674
6.333379	447.182201	10.344679
6.071686	431.767361	10.349683
6.006283	427.363969	10.354688
5.460189	441.403465	10.359693
5.742329	455.035712	10.364698
5.829255	463.555053	10.369703
5.626483	466.798870	10.374707
5.784243	463.274144	10.379712
5.983140	476.527145	10.384717
6.203002	477.551998	10.389722
6.479059	484.869359	10.394727
6.117383	492.996308	10.399731
6.327820	492.128108	10.404736
6.301957	494.110063	10.409741
6.658164	493.365285	10.414746
6.624996	490.242356	10.419751
6.350658	493.345297	10.424755
6.508201	493.033647	10.429760
6.378345	500.291933	10.434765
6.669960	516.065561	10.439770
6.923245	529.383884	10.444775
7.068202	534.850388	10.449779
7.228954	526.634629	10.454784
6.773189	523.587310	10.459789
7.136852	533.166439	10.464794
7.320432	530.875521	10.469799
6.989873	542.616384	10.474803
7.236463	531.329161	10.479808
7.218252	536.610886	10.484813
7.089498	537.875906	10.489818
7.208512	530.926077	10.494823
7.103277	538.832639	10.499827
7.544551	539.391258	10.504832
7.416376	547.465567	10.509837
7.438745	546.348172	10.514842
7.595921	548.194937	10.519847
7.178544	549.435632	10.524851
7.182184	546.110597	10.529856
7.098445	553.953483	10.534861
7.348671	557.657263	10.539866
7.578261	572.129123	10.544871
7.756555	576.567587	10.549875
8.163686	570.891459	10.554880
7.855690	575.826580	10.559885
7.910039	569.651614	10.564890
7.940093	573.704981	10.569895
8.143120	585.188998	10.574899
8.114745	576.404080	10.579904
7.980069	580.235438	10.584909
8.062553	579.633507	10.589914
8.130423	589.485224	10.594919
8.228310	588.444085	10.599923
8.550050	580.357402	10.604928
8.184082	578.166228	10.609933
8.145337	581.730882	10.614938
7.900826	587.519174	10.619943
7.800644	589.689536	10.624947
8.239312	584.111809	10.629952
7.779245	596.705815	10.634957
8.161882	615.491088	10.639962
8.214126	620.994834	10.644967
8.364875	629.537268	10.649971
8.703496	630.302566	10.654976
8.860261	631.812315	10.659981
8.666819	625.238115	10.664986
8.796486	631.453307	10.669991
8.638986	634.315195	10.674995
8.996782	625.085100	10.680000
8.641757	626.809307	10.685005
8.793570	645.270255	10.690010
8.998523	654.477603	10.695015
9.083549	652.428165	10.700019
9.408097	657.222882	10.705024
9.261997	664.591001	10.710029
9.409756	658.929314	10.715034
9.704564	663.787947	10.720039
9.519146	669.393641	10.725043
9.561871	649.925433	10.730048
9.327713	640.824061	10.735053
9.051509	647.709624	10.740058
8.993676	652.010969	10.745063
9.329731	663.551970	10.750067
9.401578	664.336168	10.755072
9.230947	670.758387	10.760077
9.778674	670.171812	10.765082
9.679549	670.258633	10.770087
9.218262	678.450518	10.775091
9.179357	671.047715	10.780096
9.536412	695.450892	10.785101
9.863426	699.233512	10.790106
10.064790	704.593300	10.795111
10.093707	706.206686	10.800115
10.461140	699.355107	10.805120
10.561872	717.866741	10.810125
10.454311	702.550729	10.815130
10.291916	688.166219	10.820135
9.916578	684.631008	10.825139
10.240470	674.730528	10.830144
10.019679	685.889007	10.835149
9.953350	699.380695	10.840154
10.230017	703.061818	10.845159
10.084262	710.225035	10.850163
10.083550	711.892054	10.855168
10.305436	715.142845	10.860173
10.277170	707.474917	10.865178
10.464920	714.725424	10.870183
10.234062	718.237787	10.875187
10.574562	734.578770	10.880192
10.857145	740.988440	10.885197
10.907158	739.463273	10.890202
10.952317	742.730951	10.895207
10.921881	745.395419	10.900211
10.947056	732.982353	10.905216
10.656990	745.331018	10.910221
10.767831	743.883051	10.915226
11.044090	732.650990	10.920231
10.714983	744.582015	10.925235
10.992052	746.056148	10.930240
10.697408	747.726200	10.935245
10.916919	753.295259	10.940250
11.221464	753.974828	10.945255
11.088170	750.103239	10.950259
11.155128	759.736539	10.955264
11.041618	774.891878	10.960269
11.595492	782.456609	10.965274
11.556707	781.277447	10.970279
11.357635	783.867417	10.975283
11.607726	780.898753	10.980288
11.751523	786.047391	10.985293
11.781394	778.528536	10.990298
12.021247	791.393079	10.995303
11.659687	786.513793	11.000307
11.554392	783.458039	11.005312
11.853397	796.214550	11.010317
11.633311	788.367106	11.015322
12.027740	783.695695	11.020327
11.747577	785.201429	11.025331
11.972583	786.131476	11.030336
11.638653	790.953480	11.035341
11.446562	791.453734	11.040346
11.853439	789.058967	11.045351
12.077424	805.148032	11.050355
12.611350	802.905555	11.055360
12.525774	796.073976	11.060365
12.371503	794.198967	11.065370
12.418363	789.924248	11.070375
12.573238	790.940529	11.075379
12.589790	794.955611	11.080384
12.350804	797.646372	11.085389
12.340148	789.558943	11.090394
12.707739	790.802038	11.095399
12.207294	788.169292	11.100403
12.756463	799.665960	11.105408
12.762124	814.897219	11.110413
12.775882	821.864192	11.115418
12.970444	822.802619	11.120423
12.959969	823.727255	11.125427
13.036084	807.317425	11.130432
12.549801	806.767217	11.135437
12.667810	813.836310	11.140442
12.831801	816.254299	11.145447
12.930213	822.110195	11.150451
13.122651	821.302695	11.155456
13.083543	819.810958	11.160461
13.334222	823.961560	11.165466
13.163830	823.288901	11.170471
12.797382	828.215175	11.175475
13.082099	826.753177	11.180480
12.930856	831.659132	11.185485
12.908077	826.245701	11.190490
13.179362	840.650663	11.195495
13.139268	863.553929	11.200499
13.682182	853.945384	11.205504
13.406617	856.487297	11.210509
13.197681	858.325426	11.215514
13.341405	852.377785	11.220519
13.534694	859.248467	11.225523
13.690979	859.251629	11.230528
13.205990	865.545065	11.235533
13.689880	881.470437	11.240538
14.111087	876.107178	11.245543
14.221290	878.191376	11.250547
14.880418	876.991227	11.255552
14.755313	863.911068	11.260557
14.316476	859.044614	11.265562
14.379848	858.419108	11.270567
14.413404	865.336523	11.275571
14.370138	851.728400	11.280576
14.821419	852.367421	11.285581
14.768931	851.610598	11.290586
14.392968	833.315251	11.295591
13.602396	829.550022	11.300595
13.950016	840.078658	11.305600
13.929006	849.279471	11.310605
14.118694	860.006514	11.315610
14.361518	858.765246	11.320615
14.024299	864.880980	11.325619
14.314170	869.545527	11.330624
14.208689	882.301988	11.335629
14.215560	882.728263	11.340634
14.783745	887.842460	11.345639
14.746989	895.919038	11.350643
15.136063	887.359998	11.355648
14.946858	889.888294	11.360653
15.241237	892.208150	11.365658
15.501741	888.043613	11.370663
14.818551	887.319534	11.375667
15.221494	884.492010	11.380672
15.020793	890.505400	11.385677
15.135213	883.318179	11.390682
15.006175	877.317823	11.395687
15.169851	881.977169	11.400691
15.389462	879.877783	11.405696
15.355740	880.313387	11.410701
15.326211	883.524822	11.415706
15.586085	877.913701	11.420711
15.532174	889.561601	11.425715
15.442472	879.530197	11.430720
15.446094	887.282088	11.435725
15.515138	894.556979	11.440730
15.496460	877.804516	11.445735
15.459827	882.170578	11.450739
15.745115	873.125268	11.455744
15.763994	884.824236	11.460749
15.777971	882.332217	11.465754
15.636612	882.507595	11.470759
15.529243	889.155502	11.475763
16.210040	901.731771	11.480768
16.382074	920.315104	11.485773
16.192852	911.175079	11.490778
16.295644	889.577738	11.495783
15.764278	892.942718	11.500787
16.412064	880.911857	11.505792
16.054625	888.831443	11.510797
16.175706	896.215439	11.515802
16.247111	905.039654	11.520807
16.184927	921.054748	11.525811
16.358799	913.791793	11.530816
16.177598	916.680296	11.535821
16.276554	919.472607	11.540826
16.961212	910.030777	11.545831
16.359467	925.381288	11.550835
16.625280	917.979806	11.555840
16.511891	920.456028	11.560845
16.389035	913.414080	11.565850
16.732526	918.356419	11.570855
16.717539	921.634448	11.575859
16.957906	919.797154	11.580864
17.066133	921.836303	11.585869
16.773599	911.966365	11.590874
16.977848	910.565525	11.595879
16.726805	920.624498	11.600883
16.474201	917.517397	11.605888
16.856209	925.756267	11.610893
16.897723	937.912048	11.615898
17.551815	931.385427	11.620903
16.883241	942.773626	11.625907
17.352612	949.165172	11.630912
17.476141	947.716590	11.635917
17.224233	954.122072	11.640922
17.298393	942.118070	11.645927
17.271315	948.981970	11.650931
17.703037	943.715569	11.655936
17.786110	950.396375	11.660941
17.303623	942.632527	11.665946
17.573598	944.460000	11.670951
17.369017	947.059230	11.675955
17.528218	945.532295	11.680960
17.574110	953.456970	11.685965
17.635338	950.636708	11.690970
17.710025	943.438114	11.695975
17.265074	946.543949	11.700979
17.922531	957.662565	11.705984
17.984764	970.935076	11.710989
18.265678	974.768695	11.715994
18.572190	956.312766	11.720999
18.411310	945.063531	11.726003
18.437170	938.179230	11.731008
18.369388	932.568216	11.736013
18.153674	944.827711	11.741018
18.526366	933.877392	11.746023
18.367540	942.097291	11.751027
18.718338	938.377125	11.756032
18.673676	938.411582	11.761037
18.879230	940.161680	11.766042
19.004642	934.901617	11.771047
18.642334	944.905473	11.776051
18.765534	924.899311	11.781056
18.863150	912.108158	11.786061
18.458504	914.516292	11.791066
18.631856	902.118342	11.796071
18.676018	925.476591	11.801075
18.697600	936.284220	11.806080
18.950491	940.459738	11.811085
18.542853	940.193275	11.816090
18.883151	941.172643	11.821095
18.646120	939.606672	11.826099
18.559273	934.855500	11.831104
18.710548	935.889776	11.836109
18.283772	945.564820	11.841114
18.637194	946.675753	11.846119
18.542078	972.229781	11.851123
18.905634	974.002134	11.856128
18.839798	972.648386	11.861133
19.314568	974.711932	11.866138
19.278567	971.712548	11.871143
19.362304	978.509305	11.876147
19.387212	987.801010	11.881152
19.572275	993.373694	11.886157
19.643083	1004.065561	11.891162
20.062555	999.273346	11.896167
19.818834	979.656077	11.901171
19.886095	976.503594	11.906176
19.705974	975.028125	11.911181
19.821543	974.433139	11.916186
19.841675	966.139024	11.921191
19.461082	975.017882	11.926195
19.684997	966.085672	11.931200
19.934811	977.007355	11.936205
19.719169	997.001717	11.941210
20.059545	990.017678	11.946215
20.354028	998.761066	11.951219
20.260114	996.388186	11.956224
20.425664	995.494103	11.961229
20.009293	992.119803	11.966234
20.231879	990.966864	11.971239
20.313701	998.263297	11.976243
20.529794	1000.383831	11.981248
20.514755	1001.818074	11.986253
20.655347	996.460256	11.991258
20.747585	976.124996	11.996263
20.176216	971.535439	12.001267
20.149459	984.638879	12.006272
20.767354	991.977212	12.011277
20.424624	994.252374	12.016282
20.839528	994.461851	12.021287
20.797612	999.143851	12.026291
20.511222	989.243205	12.031296
20.476176	987.041021	12.036301
20.339632	1000.734086	12.041306
20.716975	1000.200400	12.046311
20.414763	1006.745580	12.051315
20.579106	997.751724	12.056320
20.331945	999.198924	12.061325
20.333905	1006.106424	12.066330
20.665407	997.036144	12.071335
20.640688	997.923365	12.076339
20.653741	1000.354631	12.081344
20.666440	995.314398	12.086349
20.472919	1008.535267	12.091354
20.561483	1004.335444	12.096359
20.585303	1011.753539	12.101363
20.695478	998.352269	12.106368
20.520651	997.341678	12.111373
20.408191	997.925785	12.116378
20.631556	1000.558228	12.121383
20.354653	1008.314066	12.126387
20.539744	1014.807277	12.131392
21.088865	1005.758891	12.136397
20.898173	1013.892712	12.141402
20.939399	998.139584	12.146407
20.640857	992.879165	12.151411
20.750071	982.374248	12.156416
20.744949	982.235743	12.161421
20.470795	980.540739	12.166426
20.679406	975.739685	12.171431
20.500935	980.891933	12.176435
20.551643	973.834804	12.181440
20.876140	975.859379	12.186445
20.621564	979.092052	12.191450
20.710313	978.776005	12.196455
20.931979	978.698483	12.201459
21.040795	982.250954	12.206464
20.888227	988.192576	12.211469
21.087894	985.253441	12.216474
21.289034	970.794101	12.221479
20.582912	968.105799	12.226483
20.353184	955.470604	12.231488
20.209888	947.685702	12.236493
20.345098	961.212534	12.241498
20.754758	976.733892	12.246503
20.177843	979.106441	12.251507
20.445943	984.263043	12.256512
20.770952	981.987679	12.261517
20.597600	991.234827	12.266522
20.848263	981.814077	12.271527
20.761554	989.504532	12.276531
20.478780	980.691952	12.281536
20.862975	973.619092	12.286541
20.551697	973.723341	12.291546
20.713516	955.580379	12.296551
20.331649	961.903936	12.301555
20.152935	958.135607	12.306560
20.375314	981.479568	12.311565
20.680780	985.112796	12.316570
20.873459	984.113011	12.321575
21.067304	990.155501	12.326579
20.445802	972.000773	12.331584
20.549917	969.381970	12.336589
20.341160	967.733781	12.341594
20.589280	974.017222	12.346599
20.439577	992.593437	12.351603
20.564077	988.076800	12.356608
20.877550	996.394169	12.361613
20.651409	987.773191	12.366618
20.396480	970.241663	12.371623
20.454417	974.652721	12.376627
20.641771	984.122624	12.381632
20.726867	984.697332	12.386637
20.478183	978.362583	12.391642
20.620502	974.712891	12.396647
20.404851	982.068611	12.401651
20.664698	984.836901	12.406656
20.949946	989.956617	12.411661
20.502769	968.876224	12.416666
20.404380	962.714660	12.421671
20.739118	977.407290	12.426675
20.697999	981.682965	12.431680
20.405574	960.588287	12.436685
20.478707	968.558035	12.441690
20.861824	974.170569	12.446695
20.751732	967.322197	12.451699
20.571714	960.725421	12.456704
20.522800	961.917575	12.461709
20.125902	968.113449	12.466714
20.424487	975.446917	12.471719
20.297486	995.980683	12.476723
20.457320	996.219683	12.481728
20.695356	992.478576	12.486733
20.341938	1001.979630	12.491738
20.681660	988.302564	12.496743
20.599705	1002.081402	12.501747
20.588610	999.301558	12.506752
21.416357	990.246067	12.511757
21.009519	984.756325	12.516762
20.677891	972.771348	12.521767
20.334212	972.161551	12.526771
20.277108	970.388281	12.531776
20.372427	973.410961	12.536781
20.261708	982.888154	12.541786
20.389009	992.862568	12.546791
20.532731	999.258260	12.551795
20.259350	1007.442966	12.556800
20.694127	1004.766279	12.561805
20.550475	1004.246526	12.566810
20.931872	996.609663	12.571815
20.769105	1006.314083	12.576819
20.579449	1002.949461	12.581824
21.165063	1001.707041	12.586829
20.706244	991.858457	12.591834
20.769830	980.022422	12.596839
20.714658	973.401077	12.601843
20.544330	971.499589	12.606848
20.602018	969.560981	12.611853
20.325363	982.546214	12.616858
20.505847	969.914884	12.621863
20.344140	976.251224	12.626867
20.313249	974.959774	12.631872
20.389914	996.154933	12.636877
20.776454	1005.389382	12.641882
21.039621	991.917280	12.646887
20.388103	982.406478	12.651891
20.383305	982.898309	12.656896
20.612300	979.562175	12.661901
20.316278	1001.072293	12.666906
21.027709	998.333962	12.671911
20.099438	996.404926	12.676915
20.386397	1010.141044	12.681920
21.002762	1004.585992	12.686925
20.539180	1014.286731	12.691930
20.976300	1000.533349	12.696935
20.395133	990.611007	12.701939
20.272804	981.324866	12.706944
20.556306	997.257479	12.711949
20.650228	1011.683932	12.716954
20.855699	1002.833810	12.721959
20.543783	992.212015	12.726963
20.605025	973.037464	12.731968
20.581153	984.011208	12.736973
20.510216	989.905282	12.741978
20.658540	997.335576	12.746983
20.770909	983.171708	12.751987
20.861557	985.263616	12.756992
20.956720	981.475166	12.761997
20.854348	983.750957	12.767002
20.921144	975.218311	12.772007
21.149832	976.191949	12.777011
20.645580	984.575306	12.782016
20.517653	980.087741	12.787021
20.516448	980.099353	12.792026
20.505716	974.206964	12.797031
20.637000	976.386640	12.802035
20.648996	982.500570	12.807040
20.833670	985.462143	12.812045
20.681148	982.847472	12.817050
20.770882	982.479940	12.822055
20.785627	983.148025	12.827059
20.702525	971.760304	12.832064
20.683366	961.501227	12.837069
20.222775	960.265689	12.842074
20.358217	949.898797	12.847079
20.554503	970.017891	12.852083
20.404333	982.255520	12.857088
20.651601	980.861113	12.862093
20.341821	987.343636	12.867098
20.507059	979.554764	12.872103
20.448398	985.426995	12.877107
20.415231	988.063157	12.882112
20.396566	975.773861	12.887117
20.497732	989.794053	12.892122
20.695689	984.481272	12.897127
20.532372	986.691724	12.902131
20.321651	988.018596	12.907136
20.467633	994.192452	12.912141
20.345872	988.209753	12.917146
20.411615	989.439882	12.922151
20.493255	992.048466	12.927155
20.529861	985.857431	12.932160
20.640017	984.815742	12.937165
20.548414	991.914540	12.942170
20.817472	990.175740	12.947175
20.605283	990.203000	12.952179
20.390967	986.726952	12.957184
20.413542	991.066315	12.962189
20.312725	991.145137	12.967194
20.486270	988.386927	12.972199
20.208225	995.150984	12.977203
20.573450	1014.418146	12.982208
20.775104	1018.877601	12.987213
20.745852	1012.059953	12.992218
20.571337	997.445130	12.997223
20.609074	996.267831	13.002227
20.719909	997.080099	13.007232
20.660253	994.688713	13.012237
20.641361	1000.360710	13.017242
20.738802	990.398200	13.022247
20.673589	999.950496	13.027251
20.446360	999.704415	13.032256
20.759937	991.049316	13.037261
20.704941	996.972239	13.042266
20.767037	1002.606667	13.047271
20.564060	996.523811	13.052275
20.311147	995.797003	13.057280
20.433357	998.112053	13.062285
20.669348	994.907347	13.067290
20.667484	992.394737	13.072295
20.703011	1004.013177	13.077299
20.583798	1003.618708	13.082304
20.827828	990.155810	13.087309
20.574356	999.563937	13.092314
20.572841	995.721796	13.097319
20.801075	994.019995	13.102323
20.616049	993.407863	13.107328
20.898441	988.442182	13.112333
20.651009	993.023628	13.117338
20.744527	989.805061	13.122343
20.590360	1000.092212	13.127347
20.349025	996.396190	13.132352
20.745456	994.487130	13.137357
20.300671	1009.660417	13.142362
20.717583	999.620231	13.147367
20.836572	999.768734	13.152371
20.568716	996.538706	13.157376
20.571545	993.320688	13.162381
20.527326	992.524151	13.167386
20.588640	992.938332	13.172391
20.333208	1001.794561	13.177395
20.313082	1005.490724	13.182400
20.702612	995.139842	13.187405
20.611164	1007.447553	13.192410
20.696566	1002.913931	13.197415
21.125684	997.923879	13.202419
20.871231	1010.418620	13.207424
20.695001	1001.285393	13.212429
20.849099	1001.407745	13.217434
20.757843	988.281808	13.222439
20.996785	978.684649	13.227443
20.674740	982.128231	13.232448
20.822522	982.531928	13.237453
20.398577	980.701950	13.242458
20.732554	974.288618	13.247463
20.871979	976.144400	13.252467
20.675064	983.137303	13.257472
20.851679	972.365838	13.262477
20.486169	977.926337	13.267482
20.817409	974.378463	13.272487
20.566770	973.568372	13.277491
20.610206	983.454528	13.282496
20.558467	976.435094	13.287501
20.756619	975.791606	13.292506
20.435943	973.318662	13.297511
20.507048	977.314570	13.302515
20.457073	984.759120	13.307520
20.419855	985.525325	13.312525
19.898095	983.924880	13.317530
20.199839	974.139324	13.322535
20.325107	978.546733	13.327539
19.987406	980.571558	13.332544
20.540737	995.569751	13.337549
20.574600	1004.746248	13.342554
20.579071	1009.770823	13.347559
20.791396	1017.440021	13.352563
20.626181	1015.158704	13.357568
20.808878	1001.096445	13.362573
20.621408	991.856993	13.367578
20.575036	984.874136	13.372583
20.508100	983.102945	13.377587
20.633466	986.562580	13.382592
20.742746	973.396352	13.387597
20.584893	980.138610	13.392602
20.705828	989.831483	13.397607
20.660811	980.314982	13.402611
20.767595	978.776506	13.407616
20.658923	979.386804	13.412621
20.415032	989.972752	13.417626
20.660456	979.521456	13.422631
20.784694	980.526425	13.427635
20.738810	986.896200	13.432640
20.853715	971.934147	13.437645
20.469652	979.340845	13.442650
20.606819	984.778844	13.447655
20.466680	976.053126	13.452659
20.295288	985.212304	13.457664
20.664187	978.896008	13.462669
20.631806	989.148849	13.467674
20.414424	986.154510	13.472679
20.198088	987.341820	13.477683
20.052417	990.360823	13.482688
20.482789	990.035149	13.487693
20.597410	1009.934613	13.492698
20.810003	1012.392458	13.497703
20.714237	1000.013731	13.502707
20.496520	989.359997	13.507712
20.868239	979.891649	13.512717
20.553110	989.352183	13.517722
20.582255	982.614931	13.522727
20.604688	987.969971	13.527731
20.657672	989.155709	13.532736
20.798296	989.675501	13.537741
20.732946	992.067709	13.542746
20.503029	985.164479	13.547751
20.603492	986.958258	13.552755
20.402045	986.886177	13.557760
20.805748	990.293353	13.562765
20.630924	987.998293	13.567770
20.841446	987.988997	13.572775
20.763254	986.298288	13.577779
20.597829	993.623296	13.582784
20.667617	984.400924	13.587789
20.808990	985.708480	13.592794
20.920151	986.828585	13.597799
20.553444	984.594057	13.602803
20.368110	995.019179	13.607808
20.562606	987.422655	13.612813
20.588654	994.827334	13.617818
20.556140	994.232868	13.622823
20.712489	1000.394292	13.627827
20.771218	996.396559	13.632832
20.802440	993.400646	13.637837
20.251820	1001.413805	13.642842
20.480174	996.486992	13.647847
20.412380	1003.222503	13.652851
20.124791	1003.147428	13.657856
20.843922	987.779788	13.662861
20.645373	1000.451646	13.667866
20.969344	999.749874	13.672871
20.891921	996.092459	13.677875
20.465630	996.377085	13.682880
20.739964	994.010935	13.687885
20.625233	1001.077386	13.692890
20.788859	988.046301	13.697895
20.849925	986.594215	13.702899
20.424665	970.741886	13.707904
20.750405	965.117467	13.712909
20.558075	961.640024	13.717914
20.009234	961.353954	13.722919
20.481458	974.166176	13.727923
20.515751	986.533627	13.732928
20.705902	987.123086	13.737933
20.565704	999.786122	13.742938
20.586944	990.292992	13.747943
20.849481	991.228065	13.752947
20.770826	1001.608058	13.757952
20.712808	976.878308	13.762957
20.375395	972.537978	13.767962
20.415328	961.627324	13.772967
20.634650	974.390145	13.777971
20.577122	989.113727	13.782976
21.051569	986.388004	13.787981
20.755674	981.279504	13.792986
20.837378	966.494858	13.797991
20.722218	962.041819	13.802995
20.504042	976.104515	13.808000
20.442056	963.151212	13.813005
20.071359	966.804448	13.818010
20.323007	958.452090	13.823015
20.500007	969.516909	13.828019
20.554373	987.505501	13.833024
20.709117	989.051553	13.838029
20.299729	985.024743	13.843034
20.334825	990.891559	13.848039
20.514797	997.613797	13.853043
20.491153	998.313728	13.858048
20.973383	1000.770734	13.863053
20.773816	997.688470	13.868058
20.644658	988.820337	13.873063
21.025126	989.477822	13.878067
20.565705	981.504342	13.883072
20.482271	960.209621	13.888077
20.303686	972.741060	13.893082
20.589423	969.273226	13.898087
20.728188	970.846884	13.903091
20.286466	975.934136	13.908096
20.868885	976.969098	13.913101
20.333279	983.694416	13.918106
20.521639	991.480210	13.923111
20.707673	991.259587	13.928115
20.805676	987.011571	13.933120
20.621561	974.450645	13.938125
20.498591	970.139864	13.943130
20.641581	968.515049	13.948135
20.713882	962.532244	13.953139
20.250360	971.502292	13.958144
20.295432	963.375613	13.963149
20.745539	987.438823	13.968154
20.728956	993.453446	13.973159
20.663997	979.880904	13.978163
20.592431	980.001290	13.983168
21.060167	963.260861	13.988173
20.640524	972.689569	13.993178
20.582654	964.869485	13.998183
20.663621	972.661446	14.003187
20.726500	971.504706	14.008192
21.246237	968.347744	14.013210
20.977273	964.962084	14.018227
20.634931	970.521907	14.023245
20.871840	962.623221	14.028263
20.608408	970.185401	14.033280
20.723478	960.155884	14.038298
20.787915	971.252253	14.043315
20.533022	968.433117	14.048333
20.718593	973.144500	14.053351
20.582667	975.530920	14.058368
20.860958	963.238220	14.063386
20.399480	965.445794	14.068403
20.230634	969.469466	14.073421
20.183637	966.663114	14.078439
20.346217	971.067787	14.083456
20.661311	983.202365	14.088474
20.784526	995.654124	14.093491
20.797765	999.821794	14.098509
21.042639	1001.420434	14.103527
20.804647	1007.816377	14.108544
20.801712	998.950456	14.113562
20.779392	1010.031017	14.118579
20.724404	1006.393291	14.123597
21.144094	1002.698590	14.128615
20.893513	1004.527072	14.133632
21.356227	1000.338739	14.138650
21.220108	1008.127945	14.143667
21.098087	1011.489222	14.148685
21.141082	1002.199646	14.153703
20.778161	1014.019760	14.158720
20.915074	1012.746153	14.163738
20.996659	1007.606951	14.168755
20.999534	1003.356505	14.173773
21.017123	1003.968058	14.178791
20.855467	1008.756310	14.183808
21.085897	1006.363834	14.188826
21.146608	1000.582104	14.193843
20.795032	1002.880297	14.198861
21.096399	1009.936966	14.203879
21.435187	1028.184888	14.208896
21.001966	1032.783471	14.213914
21.319767	1031.874153	14.218931
21.054656	1034.789067	14.223949
21.368521	1036.167993	14.228967
21.109468	1045.240593	14.233984
21.395407	1033.821001	14.239002
21.380924	1040.695601	14.244019
21.350157	1041.412698	14.249037
21.888539	1035.197060	14.254055
21.489767	1046.703243	14.259072
21.602633	1041.929560	14.264090
21.612393	1038.748476	14.269107
21.662845	1041.963643	14.274125
22.087822	1034.734303	14.279143
21.648313	1036.078608	14.284160
21.640607	1032.524902	14.289178
21.554947	1028.076227	14.294195
21.438764	1036.807374	14.299213
21.873801	1033.664406	14.304231
21.823860	1031.484183	14.309248
21.683248	1020.520835	14.314266
21.426884	1008.426470	14.319283
21.590382	1037.798565	14.324301
21.204348	1033.999466	14.329319
21.168974	1036.743879	14.334336
21.025993	1040.233568	14.339354
21.534492	1044.789990	14.344371
21.417524	1037.299606	14.349389
21.793611	1053.986717	14.354407
22.171009	1063.896338	14.359424
21.893603	1055.406603	14.364442
22.187767	1038.715913	14.369459
21.690573	1037.845929	14.374477
21.895699	1024.753067	14.379495
21.648959	1038.331755	14.384512
21.696429	1057.564374	14.389530
21.962493	1061.405225	14.394547
22.070392	1067.672196	14.399565
22.255593	1055.536734	14.404583
22.378227	1066.315689	14.409600
22.373082	1053.130500	14.414618
22.313964	1027.476494	14.419635
22.046217	1039.494891	14.424653
22.311397	1029.339978	14.429671
22.137201	1032.041652	14.434688
22.212656	1026.605441	14.439706
22.515722	1024.861580	14.444723
22.176725	1033.975048	14.449741
22.175651	1023.566949	14.454759
22.102389	1033.080556	14.459776
22.107293	1033.103690	14.464794
22.433926	1033.509489	14.469811
21.969554	1031.470014	14.474829
22.180126	1032.329996	14.479847
22.073293	1028.014096	14.484864
22.046835	1036.418418	14.489882
22.052834	1046.124364	14.494899
22.215607	1064.615909	14.499917
23.144228	1058.340441	14.504935
22.828206	1050.531002	14.509952
22.649908	1037.881851	14.514970
22.578037	1027.076802	14.519987
22.314111	1038.896498	14.525005
22.591723	1030.512024	14.530023
22.310135	1027.879751	14.535040
22.536542	1037.654602	14.540058
22.696767	1033.171248	14.545075
22.299233	1038.644882	14.550093
22.739297	1033.160328	14.555111
22.801159	1029.150961	14.560128
22.399769	1033.916934	14.565146
22.524878	1033.917884	14.570163
22.133276	1037.591943	14.575181
22.386023	1046.914612	14.580199
22.623732	1065.123998	14.585216
22.486885	1073.056286	14.590234
22.742779	1062.274549	14.595251
22.153454	1077.515673	14.600269
22.754505	1071.077056	14.605287
22.454993	1068.445880	14.610304
22.455310	1079.093837	14.615322
22.730102	1073.863608	14.620339
22.705554	1075.860839	14.625357
22.884543	1087.675109	14.630375
22.783704	1103.347110	14.635392
22.937536	1109.349904	14.640410
23.127332	1105.109511	14.645427
22.993633	1096.927817	14.650445
23.115495	1094.661825	14.655463
23.400443	1085.386626	14.660480
23.248851	1076.842235	14.665498
23.547576	1063.147027	14.670515
23.527222	1072.047604	14.675533
23.276607	1061.462169	14.680551
23.198222	1073.784371	14.685568
23.121228	1071.379236	14.690586
23.327672	1065.556746	14.695603
23.199357	1072.700503	14.700621
22.910020	1065.673549	14.705639
23.301235	1067.432159	14.710656
22.945222	1069.416925	14.715674
23.459460	1073.432568	14.720691
23.117219	1070.366165	14.725709
23.192311	1060.847018	14.730727
23.341081	1067.491263	14.735744
23.206586	1069.462459	14.740762
22.933243	1058.488374	14.745779
22.890837	1073.166395	14.750797
23.501703	1071.350069	14.755815
23.700401	1067.999566	14.760832
23.563668	1071.124383	14.765850
23.631327	1072.069505	14.770867
23.348111	1076.215184	14.775885
23.501642	1075.643895	14.780903
23.432983	1074.188190	14.785920
23.525283	1078.054508	14.790938
23.483216	1070.014610	14.795955
22.986781	1066.710452	14.800973
23.231564	1086.662876	14.805991
23.383780	1097.830119	14.811008
23.359666	1102.683013	14.816026
23.447033	1103.320010	14.821043
23.593044	1100.406520	14.826061
23.438475	1099.566377	14.831079
23.713279	1104.703873	14.836096
23.407293	1103.093172	14.841114
23.713496	1092.605568	14.846131
23.362961	1095.873750	14.851149
23.640601	1096.075730	14.856167
23.923766	1107.077603	14.861184
23.690586	1100.105183	14.866202
24.076177	1105.913896	14.871219
23.610707	1110.323134	14.876237
24.058286	1117.418174	14.881255
24.262009	1109.331389	14.886272
24.050782	1099.606566	14.891290
24.306233	1085.986086	14.896307
24.102162	1088.901964	14.901325
24.131848	1080.290660	14.906343
23.979116	1081.937401	14.911360
24.065852	1080.655855	14.916378
24.383779	1082.279777	14.921395
24.419906	1088.029494	14.926413
24.285929	1077.234665	14.931431
24.254325	1088.164106	14.936448
23.745142	1087.879291	14.941466
24.301178	1083.680448	14.946483
24.290393	1082.554216	14.951501
23.995899	1085.734828	14.956519
24.255826	1089.612962	14.961536
24.092227	1091.591514	14.966554
24.124562	1086.154801	14.971571
24.301358	1092.028050	14.976589
24.353552	1083.020335	14.981607
24.248604	1079.039162	14.986624
23.988211	1086.940273	14.991642
24.473616	1081.133732	14.996659
24.523944	1083.099621	15.001677
24.257691	1088.377521	15.006695
24.236198	1081.910588	15.011712
24.321902	1104.397983	15.016730
24.451127	1106.950395	15.021747
24.728642	1118.367057	15.026765
24.625682	1108.818168	15.031783
24.802503	1092.609386	15.036800
24.490009	1098.460615	15.041818
24.666802	1091.400190	15.046835
24.554913	1082.121767	15.051853
24.754702	1086.384649	15.056871
24.881373	1086.258156	15.061888
24.876382	1084.501354	15.066906
24.952680	1080.984813	15.071923
24.576224	1084.225543	15.076941
24.485577	1075.349419	15.081959
24.453645	1075.755276	15.086976
24.401662	1099.670315	15.091994
24.762223	1100.914459	15.097011
24.836981	1112.031996	15.102029
25.021387	1115.002934	15.107047
25.145620	1111.062386	15.112064
25.210286	1114.786589	15.117082
25.023153	1113.762644	15.122099
25.027867	1103.210180	15.127117
25.009452	1099.268894	15.132135
24.859968	1079.379563	15.137152
24.665441	1098.983671	15.142170
24.893817	1106.580500	15.147187
25.216819	1106.106934	15.152205
24.808035	1112.003027	15.157223
25.400042	1114.969833	15.162240
25.107499	1112.315799	15.167258
25.196219	1112.341887	15.172275
25.300929	1120.090251	15.177293
25.058185	1116.423269	15.182311
25.253212	1105.060554	15.187328
25.142413	1118.250226	15.192346
25.263637	1111.360749	15.197363
25.241910	1110.361204	15.202381
25.170948	1120.539876	15.207399
25.085267	1108.133863	15.212416
25.173070	1118.495566	15.217434
25.229493	1113.622081	15.222451
25.300895	1118.642476	15.227469
25.252375	1116.704143	15.232487
25.657327	1116.347639	15.237504
25.518155	1119.331534	15.242522
25.389732	1115.934343	15.247539
25.358051	1117.875319	15.252557
25.150467	1117.645099	15.257575
25.163639	1110.732019	15.262592
25.367444	1125.685616	15.267610
25.420738	1134.019620	15.272627
25.727849	1136.060002	15.277645
25.419928	1142.328214	15.282663
25.756052	1141.783494	15.287680
25.935518	1141.696771	15.292698
26.404993	1146.935167	15.297715
26.181341	1125.362294	15.302733
25.847449	1125.131287	15.307751
25.927553	1125.434071	15.312768
25.774394	1122.293897	15.317786
25.854019	1121.564791	15.322803
25.606436	1114.205434	15.327821
25.628989	1118.958592	15.332839
25.976595	1110.921552	15.337856
25.680743	1117.272337	15.342874
25.480776	1115.086720	15.347891
25.834458	1122.123841	15.352909
25.402460	1130.443797	15.357927
25.656810	1131.592760	15.362944
25.889552	1130.499185	15.367962
25.945317	1134.291460	15.372979
26.045552	1136.040908	15.377997
25.367979	1132.417371	15.383015
26.234211	1138.267319	15.388032
26.118014	1148.932938	15.393050
26.265775	1143.529569	15.398067
26.257100	1132.977019	15.403085
26.156460	1142.435539	15.408103
26.007571	1136.020744	15.413120
26.198893	1148.004219	15.418138
25.919723	1159.590773	15.423155
26.181340	1164.108059	15.428173
26.246348	1165.876937	15.433191
26.224218	1168.202533	15.438208
26.158574	1164.413041	15.443226
26.272853	1167.728324	15.448243
26.286742	1167.237671	15.453261
25.997734	1175.358711	15.458279
26.449269	1170.239890	15.463296
26.518888	1165.502327	15.468314
26.576137	1168.643121	15.473331
26.850335	1156.017873	15.478349
26.120363	1168.841270	15.483367
26.614304	1167.841109	15.488384
26.595886	1167.578849	15.493402
26.629594	1163.895561	15.498419
26.586700	1160.780964	15.503437
26.656722	1169.649958	15.508455
26.746065	1167.136755	15.513472
26.799320	1159.237567	15.518490
26.945821	1161.814981	15.523507
27.235594	1155.623810	15.528525
27.051672	1151.488035	15.533543
27.116364	1150.542574	15.538560
27.262239	1157.104275	15.543578
26.867334	1155.702531	15.548595
27.040848	1150.420344	15.553613
27.003472	1160.029852	15.558631
27.012716	1155.715276	15.563648
27.195433	1158.532562	15.568666
27.406379	1155.801645	15.573683
27.501816	1151.882954	15.578701
27.109027	1141.842749	15.583719
26.562920	1128.319504	15.588736
26.613774	1134.920718	15.593754
26.784293	1152.705078	15.598771
27.306272	1149.163685	15.603789
27.120711	1158.693867	15.608807
27.278476	1159.540862	15.613824
27.521061	1156.955319	15.618842
27.320539	1156.245896	15.623859
27.463147	1153.381015	15.628877
27.132555	1158.529407	15.633895
27.415023	1157.337140	15.638912
27.617782	1157.744102	15.643930
27.011267	1159.866324	15.648947
27.425301	1146.234352	15.653965
26.945226	1155.505947	15.658983
27.124644	1154.536090	15.664000
27.190229	1150.479199	15.669018
27.328165	1154.214473	15.674035
27.446573	1149.677228	15.679053
27.194256	1160.989866	15.684071
27.363724	1163.754697	15.689088
27.397330	1157.351520	15.694106
27.376641	1180.656151	15.699123
28.051695	1179.055598	15.704141
27.748804	1173.702318	15.709159
27.663498	1165.997370	15.714176
27.707616	1164.114807	15.719194
27.484233	1180.629224	15.724211
28.118445	1179.408933	15.729229
27.611879	1171.465554	15.734247
28.028775	1174.906527	15.739264
27.947991	1163.543023	15.744282
27.540504	1162.512757	15.749299
27.998133	1158.230759	15.754317
27.573149	1170.292359	15.759335
28.000019	1186.575205	15.764352
27.752482	1185.851398	15.769370
27.880388	1186.252689	15.774387
28.003396	1180.657866	15.779405
27.583266	1193.830554	15.784423
27.772406	1188.195646	15.789440
27.971038	1188.466691	15.794458
27.690118	1186.086265	15.799475
27.828330	1186.048745	15.804493
28.066589	1192.095368	15.809511
27.973096	1184.813109	15.814528
28.140123	1194.152534	15.819546
28.481302	1214.870944	15.824563
28.666379	1193.988592	15.829581
28.513515	1190.876307	15.834599
28.291123	1189.434350	15.839616
28.387811	1184.260215	15.844634
28.327461	1187.623948	15.849651
28.357087	1189.967841	15.854669
28.305999	1190.800249	15.859687
28.086544	1181.394528	15.864704
27.920619	1188.967656	15.869722
28.214542	1208.920081	15.874739
28.210305	1210.172840	15.879757
28.564898	1225.105010	15.884775
28.607175	1220.101229	15.889792
28.849279	1209.780456	15.894810
28.695209	1224.310821	15.899827
28.950815	1218.612928	15.904845
28.839436	1218.142176	15.909863
29.153385	1218.456841	15.914880
28.894709	1207.771105	15.919898
28.528505	1192.910548	15.924915
28.720480	1196.080615	15.929933
28.926252	1212.692366	15.934951
28.857365	1206.147674	15.939968
29.086796	1192.824894	15.944986
28.569714	1190.587330	15.950003
28.549755	1193.137773	15.955021
28.931672	1209.961860	15.960039
28.932547	1221.362244	15.965056
29.099067	1209.904332	15.970074
28.873000	1219.300932	15.975091
28.868508	1212.794019	15.980109
28.764991	1217.503857	15.985127
28.813809	1215.370067	15.990144
29.315022	1209.435168	15.995162
28.954576	1208.852383	16.000179
29.013006	1220.749634	16.005197
28.923932	1213.000423	16.010215
29.272901	1212.493266	16.015232
29.174998	1207.259959	16.020250
29.163887	1207.905971	16.025267
29.291089	1207.617955	16.030285
29.365116	1206.586236	16.035303
29.196096	1211.020271	16.040320
29.399434	1214.867191	16.045338
29.190485	1209.348172	16.050355
29.332511	1211.202284	16.055373
29.319179	1213.296438	16.060391
29.165939	1209.795204	16.065408
29.240522	1214.152037	16.070426
29.410489	1239.966015	16.075443
30.135034	1224.734933	16.080461
29.927845	1221.342168	16.085479
29.858855	1210.160089	16.090496
30.355294	1200.120939	16.095514
30.122065	1209.503800	16.100531
29.883990	1204.663455	16.105549
29.967097	1202.973432	16.110567
29.741584	1207.216347	16.115584
30.037016	1204.278794	16.120602
29.629095	1202.780055	16.125619
30.358040	1206.445115	16.130637
29.746407	1188.349988	16.135655
29.534623	1198.629634	16.140672
29.528406	1195.533941	16.145690
29.281751	1204.013906	16.150707
29.574728	1195.210927	16.155725
29.700790	1200.326316	16.160743
29.661124	1208.134521	16.165760
30.073247	1208.749309	16.170778
29.665013	1209.642165	16.175795
29.879506	1221.029941	16.180813
30.102397	1229.918038	16.185831
29.986758	1234.462228	16.190848
30.148919	1225.776551	16.195866
29.891165	1231.583402	16.200883
29.941756	1239.064309	16.205901
30.077477	1235.454466	16.210919
29.711097	1233.157589	16.215936
30.159244	1227.755055	16.220954
30.095764	1235.861082	16.225971
30.416821	1248.253530	16.230989
30.578235	1252.523038	16.236007
30.326314	1245.018286	16.241024
30.808795	1233.604618	16.246042
30.654474	1226.307570	16.251059
30.426996	1240.873373	16.256077
30.821288	1229.848876	16.261095
30.540602	1226.788030	16.266112
30.967442	1226.673462	16.271130
30.520465	1226.358684	16.276147
30.822448	1229.472491	16.281165
30.887164	1229.130616	16.286183
30.599088	1231.674669	16.291200
30.424378	1229.711103	16.296218
30.607446	1224.495369	16.301235
30.710616	1226.594355	16.306253
30.432984	1228.331429	16.311271
30.409786	1236.906575	16.316288
30.726204	1237.798427	16.321306
30.876332	1255.015878	16.326323
30.916292	1261.990700	16.331341
30.966501	1256.152009	16.336359
30.799636	1264.985288	16.341376
31.278358	1255.594474	16.346394
30.898975	1258.936538	16.351411
31.157268	1255.244252	16.356429
31.144559	1252.081151	16.361447
31.365887	1252.636127	16.366464
31.309736	1240.052096	16.371482
31.242728	1234.331944	16.376499
31.056158	1222.220721	16.381517
31.217959	1219.515149	16.386535
31.249345	1232.771887	16.391552
31.463600	1238.452926	16.396570
31.139037	1243.720795	16.401587
31.170839	1242.767186	16.406605
31.389202	1244.461351	16.411623
31.390504	1253.935534	16.416640
31.571143	1252.561490	16.421658
31.523209	1259.796678	16.426675
31.288810	1255.612831	16.431693
31.684904	1253.841972	16.436711
31.418673	1257.951318	16.441728
31.726145	1252.911507	16.446746
31.559983	1255.886275	16.451763
31.794333	1259.716471	16.456781
31.741788	1249.815908	16.461799
31.490516	1257.298969	16.466816
32.129205	1255.388869	16.471834
31.814242	1241.796363	16.476851
31.588519	1234.530453	16.481869
32.065554	1241.757915	16.486887
31.540179	1239.771392	16.491904
31.579048	1245.683310	16.496922
31.975736	1254.516425	16.501939
31.734306	1254.276256	16.506957
31.983278	1247.134481	16.511975
32.006706	1252.000138	16.516992
32.098508	1259.344056	16.522010
31.648375	1255.977582	16.527027
31.781190	1264.760661	16.532045
31.873161	1253.797431	16.537063
31.665114	1264.320201	16.542080
31.784819	1256.224515	16.547098
31.649654	1252.172487	16.552115
31.757681	1269.917692	16.557133
32.237852	1277.186762	16.562151
32.091509	1287.034342	16.567168
32.376078	1282.511487	16.572186
32.712565	1285.271327	16.577203
32.537620	1281.423374	16.582221
32.613890	1265.812413	16.587239
32.296121	1264.936850	16.592256
32.315245	1256.835179	16.597274
32.633794	1267.442876	16.602291
32.246664	1267.662766	16.607309
32.273765	1266.005175	16.612327
32.098334	1275.992787	16.617344
32.354654	1282.002093	16.622362
32.532676	1282.196351	16.627379
32.421503	1282.049607	16.632397
32.695336	1283.090114	16.637415
32.645346	1277.624138	16.642432
32.423228	1277.835029	16.647450
32.866706	1279.837483	16.652467
32.495089	1275.241685	16.657485
32.613508	1278.680309	16.662503
32.383252	1287.547306	16.667520
32.949663	1301.380540	16.672538
32.981436	1309.257262	16.677555
32.769726	1318.460892	16.682573
33.345733	1305.613289	16.687591
33.204588	1317.009744	16.692608
33.001618	1312.809863	16.697626
33.160122	1296.251222	16.702643
32.970339	1300.026971	16.707661
33.336310	1298.693594	16.712679
32.902455	1295.419604	16.717696
33.072139	1301.060666	16.722714
33.001804	1297.345574	16.727731
33.051891	1308.627338	16.732749
33.362186	1303.148011	16.737767
33.321766	1304.110104	16.742784
33.262055	1308.102157	16.747802
33.052574	1320.636024	16.752819
33.500451	1310.224388	16.757837
33.523433	1302.986677	16.762855
33.233080	1310.410315	16.767872
33.550334	1303.974196	16.772890
33.264430	1311.687650	16.777907
33.395697	1314.192104	16.782925
33.767116	1309.237383	16.787943
33.296497	1310.064948	16.792960
33.325785	1307.011182	16.797978
33.601179	1302.654476	16.802995
33.320258	1307.768807	16.808013
34.167387	1288.629678	16.813031
33.970263	1296.017639	16.818048
34.159884	1299.730306	16.823066
34.364552	1289.110360	16.828083
34.060325	1297.425034	16.833101
34.144593	1296.696305	16.838119
33.909668	1291.547098	16.843136
34.144832	1287.279978	16.848154
34.154515	1292.682305	16.853171
33.873336	1298.507371	16.858189
34.070095	1290.605167	16.863207
34.171892	1293.988765	16.868224
34.124240	1298.558722	16.873242
34.444262	1294.161687	16.878259
33.824711	1302.100073	16.883277
34.342571	1289.495939	16.888295
34.226510	1292.598750	16.893312
34.153240	1291.571807	16.898330
34.071286	1296.994571	16.903347
34.159541	1296.135620	16.908365
34.260352	1282.162315	16.913383
33.988839	1293.789392	16.918400
34.196415	1292.981643	16.923418
34.394288	1289.782036	16.928435
33.930005	1301.295699	16.933453
34.172719	1294.056148	16.938471
34.370080	1301.696977	16.943488
34.409032	1321.063284	16.948506
34.400302	1317.781366	16.953523
34.278459	1329.645430	16.958541
34.276225	1323.549539	16.963559
34.227588	1324.341767	16.968576
34.136118	1321.655978	16.973594
34.421577	1332.723372	16.978611
34.622244	1347.337138	16.983629
34.743656	1347.680881	16.988647
35.023746	1348.193104	16.993664
34.763245	1348.245601	16.998682
34.999877	1356.292360	17.003699
35.114419	1360.017914	17.008717
35.297411	1345.018557	17.013735
35.512371	1349.799826	17.018752
35.045953	1334.351140	17.023770
35.230920	1317.157567	17.028787
34.894980	1318.726285	17.033805
35.041404	1329.258802	17.038823
35.271775	1333.055050	17.043840
35.334036	1343.464593	17.048858
35.147706	1322.835135	17.053875
35.285935	1339.874389	17.058893
35.326755	1330.850763	17.063911
35.395043	1333.406967	17.068928
35.206944	1335.266116	17.073946
35.278989	1338.999738	17.078963
35.465117	1346.407848	17.083981
35.233289	1344.392243	17.088999
35.575868	1338.249433	17.094016
35.555090	1342.519886	17.099034
35.749217	1346.276284	17.104051
35.410438	1344.315240	17.109069
35.503339	1347.759435	17.114087
35.501921	1347.137925	17.119104
35.383021	1353.104101	17.124122
35.546350	1343.934648	17.129139
35.735999	1343.453623	17.134157
35.518775	1341.993835	17.139175
36.135490	1332.502930	17.144192
35.779133	1347.908722	17.149210
35.932650	1342.424369	17.154227
35.550917	1347.554029	17.159245
35.820079	1342.420748	17.164263
35.719249	1344.011369	17.169280
35.755916	1346.551735	17.174298
35.891731	1349.995660	17.179315
36.158163	1360.820645	17.184333
35.904213	1377.784254	17.189351
36.163907	1376.132839	17.194368
36.087976	1380.894695	17.199386
35.936228	1380.874209	17.204403
35.963342	1382.552750	17.209421
36.332199	1376.057749	17.214439
36.100832	1371.583953	17.219456
35.858998	1382.649655	17.224474
35.989069	1378.661971	17.229491
36.075315	1385.001687	17.234509
36.127446	1401.814015	17.239527
36.635657	1406.237907	17.244544
36.718116	1405.216148	17.249562
37.006352	1402.177420	17.254579
36.539485	1395.869797	17.259597
36.654250	1396.700948	17.264615
36.718429	1382.957871	17.269632
36.210656	1391.981180	17.274650
36.754568	1398.386935	17.279667
36.699172	1402.708226	17.284685
36.519308	1403.910002	17.289703
36.870519	1404.821885	17.294720
36.858630	1413.996036	17.299738
37.003868	1401.246624	17.304755
37.168591	1401.151010	17.309773
37.092725	1398.785399	17.314791
37.203870	1402.227266	17.319808
37.112830	1399.527215	17.324826
37.588253	1391.966590	17.329843
37.237062	1380.848915	17.334861
37.168919	1366.141832	17.339879
37.241443	1357.487988	17.344896
37.065759	1363.220180	17.349914
36.927239	1354.180041	17.354931
37.267409	1368.946698	17.359949
37.307431	1376.788179	17.364967
37.278737	1382.187666	17.369984
37.356978	1397.302437	17.375002
37.230945	1400.334925	17.380019
37.465129	1399.635219	17.385037
37.316003	1404.428136	17.390055
37.435034	1394.163780	17.395072
37.258956	1400.811102	17.400090
37.703607	1392.588366	17.405107
37.771784	1401.864935	17.410125
37.648141	1396.161521	17.415143
37.787388	1384.184485	17.420160
37.845560	1397.276913	17.425178
37.885635	1398.808337	17.430195
38.314021	1395.900321	17.435213
37.689104	1383.990911	17.440231
38.103672	1384.925004	17.445248
37.966280	1378.486876	17.450266
37.996086	1366.980629	17.455283
38.014840	1361.357154	17.460301
37.571781	1366.898947	17.465319
38.059676	1376.228747	17.470336
38.171914	1382.809305	17.475354
37.784163	1389.700809	17.480371
37.435259	1384.382118	17.485389
37.402256	1389.602015	17.490407
37.482245	1392.961418	17.495424
37.559900	1406.408027	17.500442
37.994293	1418.521706	17.505459
38.176465	1425.219437	17.510477
37.679617	1420.878161	17.515495
37.909081	1420.941937	17.520512
38.366011	1434.214870	17.525530
38.426682	1449.113390	17.530547
38.547605	1449.722600	17.535565
38.902672	1446.397574	17.540583
39.199454	1434.250169	17.545600
38.554565	1427.033592	17.550618
38.514429	1415.901147	17.555635
38.796524	1411.467271	17.560653
38.583673	1420.791246	17.565671
38.839072	1405.523486	17.570688
38.671220	1419.037398	17.575706
38.840467	1422.952426	17.580723
38.743186	1420.921224	17.585741
38.777286	1423.676630	17.590759
38.890745	1421.377777	17.595776
38.703691	1443.535225	17.600794
38.870722	1446.176496	17.605811
38.899373	1442.970828	17.610829
38.774144	1449.415339	17.615847
38.952693	1447.545130	17.620864
38.982872	1443.301695	17.625882
38.947847	1439.762423	17.630899
39.190885	1448.656642	17.635917
38.811673	1451.232892	17.640935
39.164391	1452.426438	17.645952
38.932549	1458.250979	17.650970
38.943914	1445.610319	17.655987
39.535629	1461.715177	17.661005
39.196765	1475.688423	17.666023
39.518739	1477.772765	17.671040
39.675707	1484.638640	17.676058
39.550724	1479.685502	17.681075
39.681893	1484.423300	17.686093
39.612170	1475.622895	17.691111
40.044435	1478.348631	17.696128
40.007368	1464.003094	17.701146
40.018316	1451.355021	17.706163
40.139834	1447.549513	17.711181
39.859735	1450.924205	17.716199
39.870526	1446.182075	17.721216
39.530670	1447.598312	17.726234
39.381665	1433.193641	17.731251
39.517831	1441.222233	17.736269
39.301774	1459.554373	17.741287
39.519173	1472.310084	17.746304
39.924993	1480.436179	17.751322
39.890302	1473.833537	17.756339
40.048219	1471.592415	17.761357
39.683302	1483.820746	17.766375
40.047466	1473.584001	17.771392
39.889402	1488.718901	17.776410
40.191127	1502.635102	17.781427
40.393386	1507.657599	17.786445
40.248494	1510.024374	17.791463
40.761396	1504.003888	17.796480
40.688874	1511.426498	17.801498
40.355973	1513.004951	17.806515
41.005075	1502.876830	17.811533
40.341677	1496.534350	17.816551
40.683766	1496.902078	17.821568
40.609016	1496.996750	17.826586
40.359614	1499.870076	17.831603
40.473585	1495.039366	17.836621
40.807153	1503.843678	17.841639
40.917922	1508.976753	17.846656
40.930803	1508.258287	17.851674
40.770112	1506.604125	17.856691
41.055765	1503.016157	17.861709
40.724313	1506.712296	17.866727
40.980416	1497.094914	17.871744
40.542276	1507.632098	17.876762
40.756600	1504.600116	17.881779
40.872777	1503.776529	17.886797
40.838975	1513.241138	17.891815
40.868140	1500.630063	17.896832
41.002387	1501.023582	17.901850
40.972066	1496.746407	17.906867
41.252988	1496.333202	17.911885
40.839746	1502.855858	17.916903
40.889883	1522.373269	17.921920
41.397219	1517.918069	17.926938
41.523291	1521.274718	17.931955
41.750571	1518.743715	17.936973
41.594753	1520.888326	17.941991
41.859265	1515.785317	17.947008
41.634503	1514.552025	17.952026
41.398221	1516.875409	17.957043
41.700978	1509.899902	17.962061
41.428258	1514.071851	17.967079
41.579338	1507.654296	17.972096
41.828797	1508.104842	17.977114
41.773517	1514.164513	17.982131
41.732933	1510.898647	17.987149
41.782489	1518.675172	17.992167
41.984282	1514.821236	17.997184
42.067970	1510.183529	18.002202
41.692183	1516.988382	18.007219
41.939178	1510.626830	18.012237
41.675688	1523.179568	18.017255
41.717160	1519.400367	18.022272
42.142895	1510.939843	18.027290
42.042874	1516.890245	18.032307
42.019347	1518.135311	18.037325
41.657479	1529.411086	18.042343
42.246365	1539.432799	18.047360
42.150367	1543.921738	18.052378
42.359245	1549.782179	18.057395
42.288078	1542.210462	18.062413
42.178488	1550.358025	18.067431
42.239931	1541.083472	18.072448
42.579689	1535.721073	18.077466
42.279561	1540.040657	18.082483
42.532722	1541.433976	18.087501
42.612291	1544.315874	18.092519
42.960009	1555.173125	18.097536
43.256774	1542.422819	18.102554
43.300268	1545.326258	18.107571
43.749458	1520.503285	18.112589
43.436339	1532.521964	18.117607
43.403180	1521.519758	18.122624
43.453612	1502.886295	18.127642
43.155386	1497.932142	18.132659
43.520324	1493.084392	18.137677
43.169365	1488.305442	18.142695
43.576067	1488.558144	18.147712
43.623830	1488.028205	18.152730
43.371785	1486.751556	18.157747
43.481487	1478.167657	18.162765
43.216485	1484.220750	18.167783
42.930548	1465.599722	18.172800
43.637940	1474.048557	18.177818
43.473564	1487.559570	18.182835
43.694453	1475.064872	18.187853
43.684837	1471.527536	18.192871
43.124008	1464.251248	18.197888
43.223825	1459.302098	18.202906
43.177908	1485.682293	18.207923
43.634180	1476.171169	18.212941
43.258269	1487.950948	18.217959
43.459888	1486.759526	18.222976
43.448953	1486.977129	18.227994
43.344774	1495.233196	18.233011
43.186581	1487.075577	18.238029
43.435686	1504.360595	18.243047
43.490988	1513.817016	18.248064
43.760473	1520.834106	18.253082
43.441810	1525.115520	18.258099
43.442726	1523.991975	18.263117
43.584886	1534.128864	18.268135
43.649095	1552.616233	18.273152
43.839405	1552.904068	18.278170
43.972759	1558.329382	18.283187
43.859824	1553.650956	18.288205
44.022635	1549.432002	18.293223
44.068480	1548.134198	18.298240
44.231434	1558.558908	18.303258
44.304268	1582.190660	18.308275
44.497169	1579.193443	18.313293
44.780710	1580.092922	18.318311
44.651801	1589.070679	18.323328
44.842920	1572.317945	18.328346
44.623448	1562.585189	18.333363
44.621431	1550.409387	18.338381
44.634725	1551.142577	18.343399
44.429735	1568.195252	18.348416
44.731455	1576.379014	18.353434
44.553836	1583.752347	18.358451
44.630855	1582.511014	18.363469
44.566119	1580.370262	18.368487
44.331152	1590.760844	18.373504
44.912291	1576.747841	18.378522
44.725376	1584.146787	18.383539
44.669035	1591.812357	18.388557
44.993552	1601.403795	18.393575
44.989922	1599.979415	18.398592
45.153048	1598.320911	18.403610
45.090703	1606.936834	18.408627
45.351036	1609.131775	18.413645
45.381105	1604.737117	18.418663
45.434807	1603.837218	18.423680
45.648856	1604.426530	18.428698
45.680200	1604.811314	18.433715
45.755763	1603.221372	18.438733
45.660418	1607.196380	18.443751
45.556401	1602.742813	18.448768
45.841563	1598.314659	18.453786
45.587239	1606.556365	18.458803
45.427024	1597.463499	18.463821
45.841883	1603.578047	18.468839
45.624274	1599.647555	18.473856
45.656909	1601.590163	18.478874
45.699967	1602.599386	18.483891
45.968501	1599.879387	18.488909
45.979363	1605.894286	18.493927
45.828335	1602.692617	18.498944
46.175468	1595.114123	18.503962
45.699257	1600.369130	18.508979
45.749850	1597.788871	18.513997
45.708221	1594.187697	18.519015
45.567864	1621.948636	18.524032
46.147765	1626.912724	18.529050
46.076065	1639.637027	18.534067
46.365384	1634.821098	18.539085
46.052086	1635.440976	18.544103
46.031745	1636.809141	18.549120
46.477116	1627.529742	18.554138
46.380985	1637.328772	18.559155
46.263746	1629.423141	18.564173
46.451657	1630.793399	18.569191
46.325934	1644.209328	18.574208
46.692978	1660.145802	18.579226
46.751711	1656.098618	18.584243
46.930201	1658.483995	18.589261
46.939761	1653.210851	18.594279
46.807204	1652.377139	18.599296
47.125153	1650.197541	18.604314
47.152694	1653.628204	18.609331
47.287887	1649.721080	18.614349
47.229294	1646.259432	18.619367
46.884523	1651.425770	18.624384
47.109838	1641.817515	18.629402
47.054549	1650.445640	18.634419
47.161423	1650.622965	18.639437
47.478841	1646.373146	18.644455
47.053613	1653.140072	18.649472
47.510534	1649.370328	18.654490
47.382000	1656.819542	18.659507
46.993545	1650.686974	18.664525
47.218206	1650.857492	18.669543
47.431945	1656.392300	18.674560
47.483674	1644.742704	18.679578
47.206178	1650.226285	18.684595
47.113428	1660.174766	18.689613
47.558925	1670.838936	18.694631
47.730832	1685.116573	18.699648
48.098937	1671.971603	18.704666
47.872329	1679.115164	18.709683
48.132037	1681.943365	18.714701
48.224230	1678.164092	18.719719
47.879493	1695.737379	18.724736
48.155191	1681.208476	18.729754
48.091766	1682.991165	18.734771
48.249174	1688.722673	18.739789
48.303629	1677.258433	18.744807
48.197246	1673.989639	18.749824
48.159517	1675.982120	18.754842
48.495543	1674.855052	18.759859
48.451940	1677.279692	18.764877
48.661184	1649.846168	18.769895
48.373800	1643.308041	18.774912
48.316231	1642.767414	18.779930
47.930210	1651.636516	18.784947
48.113816	1660.331968	18.789965
48.578248	1662.600990	18.794983
48.187095	1674.930041	18.800000
48.536124	1672.634862	18.805018
48.340301	1674.033905	18.810035
48.240238	1681.162070	18.815053
48.657625	1692.402794	18.820071
48.735948	1700.213065	18.825088
49.179222	1699.234950	18.830106
48.685847	1706.037601	18.835123
48.463451	1707.437265	18.840141
49.001580	1701.576178	18.845159
48.697384	1706.289856	18.850176
49.080190	1705.542213	18.855194
48.967874	1714.617602	18.860211
48.911038	1734.535160	18.865229
49.125816	1730.511996	18.870247
49.129493	1732.874594	18.875264
49.182052	1728.916255	18.880282
49.191121	1734.453108	18.885299
49.179728	1740.957364	18.890317
49.695154	1735.465949	18.895335
49.736317	1740.785859	18.900352
49.626729	1727.354196	18.905370
49.831986	1734.243796	18.910387
49.427414	1735.107306	18.915405
49.751495	1726.359728	18.920423
49.720614	1739.703959	18.925440
49.669232	1746.404861	18.930458
50.251722	1749.384845	18.935475
50.216843	1746.099446	18.940493
50.300244	1720.014305	18.945511
50.056128	1721.727179	18.950528
50.404330	1715.258811	18.955546
50.583807	1705.929667	18.960563
50.537262	1714.567353	18.965581
50.782828	1699.366355	18.970599
50.888036	1702.231287	18.975616
50.822619	1703.036647	18.980634
50.815984	1695.301805	18.985651
50.823076	1686.739321	18.990669
51.007817	1668.155870	18.995687
50.371141	1675.907199	19.000704
50.434118	1675.975502	19.005722
50.527110	1672.106319	19.010739
50.341890	1677.567395	19.015757
50.245373	1660.787101	19.020775
50.392752	1678.202759	19.025792
50.767360	1699.787446	19.030810
50.156266	1699.773658	19.035827
50.197170	1707.403712	19.040845
50.732351	1705.217574	19.045863
50.710354	1709.574961	19.050880
50.914776	1722.843004	19.055898
51.293532	1730.474994	19.060915
50.855746	1743.632663	19.065933
51.609367	1728.103163	19.070951
51.624811	1735.004832	19.075968
51.437327	1722.485059	19.080986
51.784860	1703.774038	19.086003
51.464970	1697.748213	19.091021
51.634729	1697.713159	19.096039
51.747327	1702.323483	19.101056
51.585287	1703.496238	19.106074
51.834220	1691.824214	19.111091
52.154969	1699.156650	19.116109
51.828044	1699.956446	19.121127
51.831068	1704.586739	19.126144
51.447155	1702.261295	19.131162
51.769296	1694.221631	19.136179
51.375808	1700.811856	19.141197
51.452114	1697.142007	19.146215
51.828078	1706.449856	19.151232
51.725906	1715.812517	19.156250
51.632318	1723.510525	19.161267
51.761862	1728.807403	19.166285
51.590795	1729.279262	19.171303
51.513868	1738.895514	19.176320
51.570359	1755.021567	19.181338
51.813527	1765.345644	19.186355
51.627831	1772.164478	19.191373
52.120515	1767.271117	19.196391
52.240347	1784.568373	19.201408
52.435452	1799.812729	19.206426
52.636270	1792.663213	19.211443
52.722808	1790.584696	19.216461
52.750349	1782.993970	19.221479
52.700472	1790.927853	19.226496
52.836269	1784.834104	19.231514
52.887742	1781.722497	19.236531
52.712065	1789.976804	19.241549
52.917399	1784.611774	19.246567
52.964321	1783.603566	19.251584
52.738180	1793.224565	19.256602
53.362508	1777.245473	19.261619
52.945542	1793.360602	19.266637
52.763424	1789.643689	19.271655
52.841336	1790.410305	19.276672
52.707031	1788.064497	19.281690
53.274888	1800.450511	19.286707
53.094308	1817.888296	19.291725
53.375332	1807.765601	19.296743
53.325083	1817.221008	19.301760
53.207802	1817.839967	19.306778
53.616695	1817.843451	19.311795
53.628497	1822.115930	19.316813
53.805315	1820.016813	19.321831
53.765454	1823.000351	19.326848
53.474034	1816.331331	19.331866
53.841016	1813.693642	19.336883
53.470223	1821.039569	19.341901
53.209875	1812.987887	19.346919
53.772268	1820.234456	19.351936
53.649812	1840.036217	19.356954
54.300805	1833.671025	19.361971
53.919442	1840.892379	19.366989
54.077130	1839.498989	19.372007
54.200675	1837.590127	19.377024
54.504895	1843.931247	19.382042
54.419661	1837.053617	19.387059
54.026729	1837.679674	19.392077
54.006023	1840.398088	19.397095
54.010422	1837.514254	19.402112
54.058917	1854.893512	19.407130
54.489418	1862.743102	19.412147
54.641162	1870.515670	19.417165
54.582137	1873.296966	19.422183
54.880783	1870.988741	19.427200
54.593250	1871.848729	19.432218
54.978331	1871.508614	19.437235
54.691264	1871.504239	19.442253
54.924242	1875.065105	19.447271
55.291698	1872.352513	19.452288
54.815190	1866.354655	19.457306
55.048817	1869.252332	19.462323
54.812632	1858.139403	19.467341
55.429001	1858.704636	19.472359
55.197561	1858.615123	19.477376
55.257514	1866.943259	19.482394
55.645162	1868.628158	19.487411
55.318461	1864.763159	19.492429
55.354983	1868.488037	19.497447
55.929723	1874.133887	19.502464
55.707482	1877.520405	19.507482
55.639269	1858.752116	19.512499
55.592723	1868.029731	19.517517
55.521541	1875.490084	19.522535
55.682458	1873.038916	19.527552
55.836766	1874.691765	19.532570
56.115272	1870.308383	19.537587
55.748281	1880.353240	19.542605
56.216562	1875.225418	19.547623
56.368909	1869.624925	19.552640
56.169323	1873.355634	19.557658
55.952529	1866.730891	19.562675
56.246948	1868.754257	19.567693
56.106947	1871.518723	19.572711
56.075647	1866.163524	19.577728
56.237395	1873.479990	19.582746
56.351942	1867.472146	19.587763
56.408980	1876.702476	19.592781
56.355046	1875.443803	19.597799
56.500773	1867.570534	19.602816
56.444521	1872.700078	19.607834
56.458095	1872.849696	19.612851
56.670609	1881.217439	19.617869
56.598489	1898.406769	19.622887
56.954594	1890.689570	19.627904
56.743516	1899.368561	19.632922
57.317179	1900.900690	19.637939
57.184975	1903.034610	19.642957
57.130786	1892.736231	19.647975
57.302387	1886.882399	19.652992
56.939145	1894.279828	19.658010
57.038396	1894.352938	19.663027
56.970785	1897.360542	19.668045
57.275229	1888.829261	19.673063
56.985513	1890.275132	19.678080
57.438061	1894.290547	19.683098
57.418787	1890.685865	19.688115
57.459016	1895.986301	19.693133
57.037432	1901.986468	19.698151
57.785000	1903.178505	19.703168
57.751454	1921.676770	19.708186
57.651676	1925.329349	19.713203
57.987776	1923.959306	19.718221
57.613456	1924.812520	19.723239
57.985673	1927.516346	19.728256
57.518432	1923.923491	19.733274
57.620134	1919.804690	19.738291
57.832792	1926.998659	19.743309
58.011965	1930.603806	19.748327
58.442548	1940.582047	19.753344
58.658339	1952.617072	19.758362
58.513118	1939.322062	19.763379
57.979205	1926.658737	19.768397
58.212806	1942.225021	19.773415
58.729891	1942.092225	19.778432
58.238886	1953.091585	19.783450
58.441671	1950.319799	19.788467
58.461368	1950.139979	19.793485
58.390593	1953.146955	19.798503
58.820436	1943.478249	19.803520
58.744905	1942.027184	19.808538
58.898556	1950.590121	19.813555
58.988435	1945.851998	19.818573
58.949911	1942.973535	19.823591
59.295177	1943.537214	19.828608
58.629975	1944.293036	19.833626
59.383337	1957.328564	19.838643
58.992098	1948.021130	19.843661
59.078657	1961.095382	19.848679
59.427096	1965.480680	19.853696
59.293796	1982.374250	19.858714
59.557052	1973.622395	19.863731
59.644517	1967.589625	19.868749
59.621907	1963.926830	19.873767
59.972569	1954.239799	19.878784
60.066675	1965.306196	19.883802
60.291354	1942.946567	19.888819
60.038055	1928.513250	19.893837
60.068220	1929.410122	19.898855
60.282316	1921.328623	19.903872
59.833276	1920.665707	19.908890
60.072576	1915.458217	19.913907
60.287617	1910.417901	19.918925
59.850495	1924.291842	19.923943
60.332275	1921.256452	19.928960
59.827695	1922.939584	19.933978
59.939228	1927.254450	19.938995
59.975241	1937.505876	19.944013
59.977228	1945.945187	19.949031
60.131460	1950.913062	19.954048
60.244864	1953.034017	19.959066
60.249874	1959.609184	19.964083
60.380680	1952.298742	19.969101
60.478144	1969.462224	19.974119
60.613441	1983.308952	19.979136
60.568948	1993.148963	19.984154
60.491395	1984.694148	19.989171
60.759252	1987.029605	19.994189
60.658565	1992.695618	19.999207
60.768630	1981.180277	20.004224
60.887750	1996.529991	20.009242
60.918172	2002.150297	20.014259
61.525937	2002.843801	20.019277
61.346709	2014.068133	20.024295
61.547059	2012.274840	20.029312
61.231031	2014.111507	20.034330
61.411405	2007.593831	20.039347
61.701331	2012.763295	20.044365
61.396281	2010.429401	20.049383
61.418035	2001.062154	20.054400
61.698212	2014.291076	20.059418
61.224684	2009.343582	20.064435
61.541919	2007.807059	20.069453
61.391927	2022.987555	20.074471
61.917202	2031.071016	20.079488
61.789384	2042.852381	20.084506
62.242090	2044.571034	20.089523
62.502582	2034.422183	20.094541
62.207339	2043.908311	20.099559
62.563888	2028.825781	20.104576
62.640203	2033.936587	20.109594
62.483352	2028.989131	20.114611
62.557430	2012.084710	20.119629
62.409434	2005.225247	20.124647
62.407637	2014.604741	20.129664
62.423173	2025.683077	20.134682
62.223009	2030.599124	20.139699
62.807920	2032.213996	20.144717
62.637344	2040.392352	20.149735
62.917880	2033.109358	20.154752
62.732157	2025.890163	20.159770
62.618753	2030.051470	20.164787
62.844898	2029.282634	20.169805
62.813723	2036.039258	20.174823
62.778050	2028.680540	20.179840
62.772579	2046.661471	20.184858
63.208095	2058.132457	20.189875
63.588144	2052.504279	20.194893
63.159520	2065.793341	20.199911
63.420944	2065.578769	20.204928
63.684962	2062.553913	20.209946
63.474011	2069.750091	20.214963
63.817868	2065.913009	20.219981
63.140384	2065.756247	20.224999
63.475437	2061.835230	20.230016
63.431512	2057.392493	20.235034
63.228498	2066.465130	20.240051
63.803856	2080.321154	20.245069
63.817149	2093.520692	20.250087
63.832847	2093.649473	20.255104
63.852791	2096.930728	20.260122
63.687182	2090.711739	20.265139
63.868229	2085.415348	20.270157
63.991506	2099.902519	20.275175
64.154026	2110.375317	20.280192
64.415889	2115.090112	20.285210
64.335337	2121.402418	20.290227
64.445778	2121.305477	20.295245
64.298714	2126.612507	20.300263
64.592266	2117.987681	20.305280
64.411451	2123.142994	20.310298
64.122282	2119.427423	20.315315
64.178815	2135.497948	20.320333
64.445972	2146.892336	20.325351
64.592590	2147.745236	20.330368
64.776925	2145.617224	20.335386
64.545378	2164.684052	20.340403
65.551717	2160.683359	20.345421
65.463257	2159.803077	20.350439
65.718930	2150.412174	20.355456
65.978885	2146.996996	20.360474
65.735866	2132.952335	20.365491
66.067757	2121.046447	20.370509
66.317113	2117.552767	20.375527
66.003830	2114.577657	20.380544
66.001639	2118.322619	20.385562
65.616678	2112.583025	20.390579
66.047240	2091.624705	20.395597
65.348669	2095.124436	20.400615
66.019387	2104.478066	20.405632
66.204713	2114.113768	20.410650
66.476659	2117.297483	20.415667
66.645505	2099.334840	20.420685
66.205929	2088.301504	20.425703
66.216981	2086.840306	20.430720
66.433327	2081.273260	20.435738
65.775333	2089.441100	20.440755
66.112276	2097.842360	20.445773
66.428119	2114.247593	20.450791
66.424546	2114.974251	20.455808
66.319971	2111.666467	20.460826
66.445587	2123.570213	20.465843
66.207989	2120.005666	20.470861
65.946267	2118.799923	20.475879
66.108906	2129.254601	20.480896
66.341868	2140.694223	20.485914
66.033693	2149.152956	20.490931
66.641356	2162.492417	20.495949
66.650721	2175.572995	20.500967
66.810613	2177.087498	20.505984
66.896233	2182.484595	20.511002
66.744864	2186.321301	20.516019
66.985597	2200.049736	20.521037
67.176525	2213.981238	20.526055
67.508311	2212.465827	20.531072
67.677266	2201.688765	20.536090
67.507449	2211.905177	20.541107
67.632851	2207.679073	20.546125
67.723500	2211.686922	20.551143
67.965647	2211.610714	20.556160
68.139944	2210.795633	20.561178
67.957193	2209.770860	20.566195
67.937565	2202.546338	20.571213
67.732346	2211.276472	20.576231
67.777970	2210.483451	20.581248
67.979792	2216.218958	20.586266
68.013471	2238.636974	20.591283
68.189447	2234.160423	20.596301
68.231720	2233.012804	20.601319
68.192316	2239.612635	20.606336
68.636130	2232.779581	20.611354
68.657812	2232.471051	20.616371
68.927728	2227.710640	20.621389
69.071646	2237.295241	20.626407
68.495002	2234.358172	20.631424
68.852837	2233.484060	20.636442
69.062410	2238.184232	20.641459
69.422300	2240.270056	20.646477
69.502798	2236.491866	20.651495
69.088567	2235.300448	20.656512
69.388315	2230.562484	20.661530
68.868482	2236.619391	20.666547
69.149854	2238.631261	20.671565
69.260186	2238.064976	20.676583
69.191419	2230.672462	20.681600
69.375382	2231.032277	20.686618
69.474317	2243.740022	20.691635
69.645396	2243.809877	20.696653
69.728138	2252.928525	20.701671
69.687525	2252.572399	20.706688
69.519401	2252.392488	20.711706
69.824800	2259.226170	20.716723
70.054816	2243.019678	20.721741
70.031331	2252.343181	20.726759
69.742650	2249.471717	20.731776
70.285754	2243.524134	20.736794
69.952825	2259.279611	20.741811
70.032593	2267.472653	20.746829
70.218753	2273.454998	20.751847
70.648024	2284.829568	20.756864
70.890307	2277.682174	20.761882
70.454807	2280.269780	20.766899
70.848660	2269.410800	20.771917
70.983565	2274.116697	20.776935
70.880248	2279.604496	20.781952
71.049008	2268.647867	20.786970
70.474297	2268.045462	20.791987
70.541914	2271.001209	20.797005
71.024839	2269.952869	20.802023
70.709678	2273.005743	20.807040
71.000803	2274.465468	20.812058
70.850867	2286.831605	20.817075
71.416823	2290.846188	20.822093
71.202111	2300.052875	20.827111
71.152356	2298.846215	20.832128
71.561976	2297.015831	20.837146
71.123545	2301.165600	20.842163
71.273930	2302.711672	20.847181
71.701938	2327.190097	20.852199
71.770227	2327.050768	20.857216
72.155688	2329.230660	20.862234
72.215480	2326.786128	20.867251
72.366183	2330.089903	20.872269
72.415950	2325.736555	20.877287
72.424046	2331.792764	20.882304
72.893879	2314.795360	20.887322
72.571805	2307.384023	20.892339
72.160744	2291.630751	20.897357
72.505833	2296.339209	20.902375
72.636867	2299.243925	20.907392
72.505651	2295.867429	20.912410
72.433053	2307.061877	20.917427
72.275709	2311.315450	20.922445
73.046567	2313.753725	20.927463
72.376397	2322.274613	20.932480
72.505340	2322.595038	20.937498
72.556187	2313.250179	20.942515
72.348784	2311.698835	20.947533
72.465690	2332.494593	20.952551
72.430461	2344.752119	20.957568
72.546268	2347.397209	20.962586
72.691027	2367.856690	20.967603
72.942039	2386.636298	20.972621
73.021301	2379.458529	20.977639
72.547081	2384.459473	20.982656
73.126606	2399.241987	20.987674
73.365748	2409.802653	20.992691
73.746959	2414.272633	20.997709
74.057210	2408.653146	21.002727
73.786273	2409.086231	21.007744
74.056244	2409.049354	21.012762
74.217602	2409.633557	21.017779
74.609682	2406.906811	21.022797
74.527732	2405.422939	21.027815
74.466993	2413.987447	21.032832
74.210509	2401.949114	21.037850
74.442210	2409.244388	21.042867
74.121567	2403.814182	21.047885
74.482430	2410.675435	21.052903
74.858586	2431.756065	21.057920
75.405097	2414.759582	21.062938
74.933139	2411.049291	21.067955
74.759804	2395.905656	21.072973
75.494057	2389.107794	21.077991
74.956497	2397.227185	21.083008
75.189649	2392.419476	21.088026
75.271894	2398.461423	21.093043
75.052081	2394.936290	21.098061
75.590545	2396.363072	21.103079
75.137054	2407.496889	21.108096
75.344795	2413.226729	21.113114
75.381689	2426.142141	21.118131
75.323373	2424.164372	21.123149
75.365544	2425.250191	21.128167
75.239226	2424.515777	21.133184
75.468102	2425.708191	21.138202
75.495758	2439.997862	21.143219
75.834261	2439.034913	21.148237
76.292645	2438.759401	21.153255
76.202392	2445.701162	21.158272
76.491887	2446.928862	21.163290
76.672759	2443.356285	21.168307
76.540438	2434.299493	21.173325
76.751367	2425.613849	21.178343
76.726496	2433.522506	21.183360
76.726132	2424.751021	21.188378
76.672491	2408.977304	21.193395
76.297404	2407.893352	21.198413
76.646474	2417.768928	21.203431
76.474021	2436.120328	21.208448
76.746863	2432.379993	21.213466
76.856597	2441.196437	21.218483
76.603564	2435.427803	21.223501
76.733218	2437.233390	21.228519
76.408523	2444.967435	21.233536
76.935242	2461.000998	21.238554
77.023852	2465.870034	21.243571
76.831775	2474.007411	21.248589
77.261319	2464.541623	21.253607
77.089674	2472.559729	21.258624
77.260320	2491.833637	21.263642
77.488294	2500.148660	21.268659
77.151447	2510.153704	21.273677
77.507490	2505.950981	21.278695
77.306251	2514.385275	21.283712
77.391067	2527.719398	21.288730
77.654694	2527.396946	21.293747
77.362632	2538.736289	21.298765
78.013433	2544.624115	21.303783
78.108471	2555.893167	21.308800
78.258428	2553.942677	21.313818
78.301278	2560.072557	21.318835
78.452626	2567.839241	21.323853
78.800169	2551.272067	21.328871
78.546888	2557.540920	21.333888
78.262359	2565.773737	21.338906
78.476353	2578.014706	21.343923
78.401814	2590.387056	21.348941
79.212092	2581.878147	21.353959
79.085152	2586.877105	21.358976
79.438185	2580.848578	21.363994
79.528570	2573.443579	21.369011
79.377784	2577.498428	21.374029
80.001178	2565.958836	21.379047
79.611159	2573.904965	21.384064
79.758362	2570.536592	21.389082
79.630441	2564.077054	21.394099
79.522828	2571.112413	21.399117
79.765203	2568.478246	21.404135
79.581538	2568.339584	21.409152
79.726817	2573.158774	21.414170
79.935125	2576.759864	21.419187
79.923355	2573.925919	21.424205
80.225362	2584.809842	21.429223
80.203739	2598.662360	21.434240
80.143109	2599.865832	21.439258
80.538074	2601.577125	21.444275
80.340959	2599.764099	21.449293
80.543943	2598.649542	21.454311
80.456078	2601.010640	21.459328
80.363482	2595.359348	21.464346
80.295194	2599.537878	21.469363
80.420840	2604.703022	21.474381
80.467340	2622.242163	21.479399
80.611624	2630.488125	21.484416
80.723418	2638.104904	21.489434
81.039671	2632.838702	21.494451
81.026577	2637.282630	21.499469
81.155539	2632.470660	21.504487
81.059828	2643.683485	21.509504
81.120518	2651.548445	21.514522
81.304189	2649.334638	21.519539
81.303028	2664.303588	21.524557
81.555499	2651.009882	21.529575
81.571041	2660.805761	21.534592
81.615074	2662.589038	21.539610
81.995886	2677.438962	21.544627
81.892702	2690.864521	21.549645
82.076794	2686.577824	21.554663
82.086630	2694.790954	21.559680
82.062302	2685.895062	21.564698
82.135399	2680.555551	21.569715
81.928617	2691.469285	21.574733
82.187038	2686.580763	21.579751
82.606899	2698.996807	21.584768
82.153979	2707.478290	21.589786
82.639370	2698.748592	21.594803
82.584289	2706.245955	21.599821
82.687850	2704.286076	21.604839
82.702842	2717.153504	21.609856
82.712847	2720.636630	21.614874
83.252390	2726.538875	21.619891
83.427355	2740.238108	21.624909
83.463368	2729.883549	21.629927
83.776328	2729.933021	21.634944
83.301149	2740.655753	21.639962
83.548714	2734.321569	21.644979
83.603010	2742.127029	21.649997
83.890266	2719.441338	21.655015
83.584421	2727.678681	21.660032
83.821261	2732.160903	21.665050
83.785315	2729.362577	21.670067
83.769068	2740.661078	21.675085
84.081158	2733.401492	21.680103
84.060365	2737.207282	21.685120
84.011485	2757.680782	21.690138
84.773524	2755.504836	21.695155
84.474803	2760.934948	21.700173
84.705939	2754.406686	21.705191
84.749614	2756.413699	21.710208
84.502757	2758.689459	21.715226
84.693135	2756.546154	21.720243
84.399866	2759.789891	21.725261
84.555424	2751.916858	21.730279
84.708300	2757.057695	21.735296
84.753761	2772.499159	21.740314
84.788062	2788.548176	21.745331
84.879602	2792.819850	21.750349
85.002725	2785.832052	21.755367
85.094435	2795.759078	21.760384
85.045165	2799.244508	21.765402
85.410266	2805.153063	21.770419
85.248529	2821.319203	21.775437
85.638784	2811.648880	21.780455
86.116574	2809.976076	21.785472
85.901020	2821.549008	21.790490
86.052728	2813.439552	21.795507
85.767322	2811.636125	21.800525
86.035127	2817.786605	21.805543
85.946531	2813.901022	21.810560
86.055137	2821.398729	21.815578
86.681111	2829.477158	21.820595
86.560285	2831.597439	21.825613
86.449663	2835.993564	21.830631
86.783892	2838.024016	21.835648
86.628930	2839.288570	21.840666
87.100566	2839.594357	21.845683
87.108533	2840.573449	21.850701
87.438198	2836.577562	21.855719
87.236407	2834.006112	21.860736
87.532932	2836.755761	21.865754
87.768781	2824.531100	21.870771
87.654734	2835.714129	21.875789
87.668893	2831.945595	21.880807
87.760261	2828.489084	21.885824
87.175439	2821.387164	21.890842
87.300006	2818.286448	21.895859
87.427209	2833.564324	21.900877
87.818243	2829.432697	21.905895
87.649731	2827.895896	21.910912
87.422807	2844.228382	21.915930
87.634089	2847.492742	21.920947
87.667095	2861.031343	21.925965
87.684609	2851.061051	21.930983
87.841045	2869.509356	21.936000
87.980260	2891.996842	21.941018
88.296237	2887.807976	21.946035
88.004663	2904.613901	21.951053
88.325790	2901.571614	21.956071
88.670054	2919.086026	21.961088
88.770219	2924.515538	21.966106
88.914206	2913.246898	21.971123
89.207352	2914.409432	21.976141
89.077326	2917.360595	21.981159
89.350176	2915.236207	21.986176
89.436191	2917.814046	21.991194
89.325955	2918.747253	21.996211
89.271885	2914.642298	22.001229
89.370189	2908.348598	22.006247
90.092857	2925.272058	22.011264
90.186286	2918.535796	22.016282
90.314997	2906.921681	22.021299
90.487822	2902.300572	22.026317
90.320708	2898.641068	22.031335
90.544895	2891.146826	22.036352
90.274627	2901.073760	22.041370
90.480245	2889.273998	22.046387
90.037852	2894.718549	22.051405
90.424231	2888.699153	22.056423
90.834625	2889.602955	22.061440
90.581223	2895.549066	22.066458
90.643637	2889.141818	22.071475
90.767928	2889.819026	22.076493
90.566328	2897.499899	22.081511
90.814330	2888.920264	22.086528
90.586607	2903.741636	22.091546
90.724675	2918.382963	22.096563
90.937543	2926.121952	22.101581
90.635443	2926.108335	22.106599
90.781142	2919.758464	22.111616
90.617525	2944.999256	22.116634
91.129630	2946.968513	22.121651
91.058262	2952.770816	22.126669
90.804029	2978.672205	22.131687
91.276426	2981.996572	22.136704
91.103404	2998.793299	22.141722
91.552310	3008.147309	22.146739
91.985763	3013.910341	22.151757
91.779458	3029.355842	22.156775
92.055629	3021.247781	22.161792
92.040495	3045.402435	22.166810
92.182488	3049.623789	22.171827
92.419972	3051.392847	22.176845
92.451825	3048.622218	22.181863
92.746433	3045.021344	22.186880
92.840224	3049.563623	22.191898
92.976636	3040.668325	22.196915
92.997479	3050.904572	22.201933
92.880178	3066.853066	22.206951
93.534777	3058.287114	22.211968
93.130972	3072.053572	22.216986
93.390653	3065.441532	22.222003
93.690176	3064.304879	22.227021
93.406571	3069.341874	22.232039
93.945472	3059.489192	22.237056
94.227923	3065.043438	22.242074
94.322744	3047.571635	22.247091
94.222507	3051.088698	22.252109
94.238499	3050.136115	22.257127
94.605525	3040.852390	22.262144
94.334470	3052.921719	22.267162
94.613359	3043.417622	22.272179
94.672266	3046.960167	22.277197
94.616298	3050.842943	22.282215
94.585569	3044.290151	22.287232
94.672951	3054.391347	22.292250
94.811275	3052.349071	22.297267
94.665106	3041.717605	22.302285
94.456530	3052.930382	22.307303
94.954941	3048.178594	22.312320
94.733674	3054.806795	22.317338
94.748528	3053.181043	22.322355
94.868502	3061.683420	22.327373
94.692470	3069.770312	22.332391
94.903978	3077.981358	22.337408
94.817192	3087.484747	22.342426
94.924338	3105.675583	22.347443
95.201934	3112.994821	22.352461
95.593623	3110.294801	22.357479
95.644985	3117.118858	22.362496
95.994100	3134.498007	22.367514
96.148712	3135.267686	22.372531
96.306066	3136.355859	22.377549
96.430802	3136.526598	22.382567
96.326688	3132.490020	22.387584
96.408103	3128.620103	22.392602
96.454845	3128.701830	22.397619
96.643677	3136.432441	22.402637
96.987338	3135.550476	22.407655
96.783899	3131.463196	22.412672
96.849761	3137.735057	22.417690
97.089219	3151.224338	22.422707
97.166976	3156.252175	22.427725
97.366231	3152.508536	22.432743
97.271969	3151.123575	22.437760
97.240067	3160.891671	22.442778
97.257238	3159.111936	22.447795
97.579344	3156.851486	22.452813
97.606205	3164.682337	22.457831
98.014804	3159.701767	22.462848
97.784759	3158.209348	22.467866
97.853116	3181.475699	22.472883
97.864894	3186.269136	22.477901
97.895624	3192.073712	22.482919
98.028858	3191.195530	22.487936
98.005601	3194.256813	22.492954
98.288630	3199.744853	22.497971
98.516617	3211.121531	22.502989
98.298491	3224.968911	22.508007
98.331561	3217.000873	22.513024
98.480156	3217.619587	22.518042
98.339479	3230.625171	22.523059
99.049681	3231.975340	22.528077
99.105007	3233.755171	22.533095
99.246285	3232.357387	22.538112
98.939605	3234.466267	22.543130
99.264803	3233.916666	22.548147
99.778755	3247.351883	22.553165
99.943786	3255.831676	22.558183
99.915874	3245.329436	22.563200
99.943873	3244.564588	22.568218
100.003338	3252.539531	22.573235
100.727877	3246.561261	22.578253
100.113427	3250.878488	22.583271
100.411575	3228.669828	22.588288
100.483519	3223.490207	22.593306
100.544337	3216.470371	22.598323
100.840459	3217.949022	22.603341
100.347292	3220.693936	22.608359
100.583755	3237.610520	22.613376
100.784133	3239.043369	22.618394
100.798275	3253.360511	22.623411
100.517423	3247.017481	22.628429
100.532593	3264.251619	22.633447
100.406427	3259.264252	22.638464
100.806320	3273.238055	22.643482
100.712192	3282.834966	22.648499
101.058447	3286.666171	22.653517
101.348134	3310.679978	22.658535
101.506776	3308.067133	22.663552
101.912735	3311.417139	22.668570
101.726368	3314.056705	22.673587
101.855609	3309.164936	22.678605
101.858901	3309.715631	22.683623
101.999638	3311.059477	22.688640
101.717866	3328.800598	22.693658
101.905175	3338.049228	22.698675
102.134903	3341.360934	22.703693
102.234680	3350.107927	22.708711
102.393045	3359.422175	22.713728
102.578897	3366.086245	22.718746
102.567441	3379.235189	22.723763
103.107174	3361.452852	22.728781
103.313250	3363.046189	22.733799
103.501885	3346.956706	22.738816
103.541597	3350.179704	22.743834
103.799851	3346.872460	22.748851
104.096313	3339.375067	22.753869
104.010527	3342.242330	22.758887
103.850494	3340.459087	22.763904
104.065507	3346.732239	22.768922
103.842161	3351.379380	22.773939
104.069351	3338.723428	22.778957
103.810654	3347.227872	22.783975
103.799265	3345.731813	22.788992
103.843090	3362.382278	22.794010
103.730927	3366.219636	22.799027
104.432330	3373.903445	22.804045
104.280007	3390.964030	22.809063
104.641249	3402.623582	22.814080
104.627433	3405.602168	22.819098
104.818258	3409.689235	22.824115
104.996324	3401.463910	22.829133
104.987841	3402.755375	22.834151
105.229006	3409.202061	22.839168
105.388404	3404.490174	22.844186
105.153193	3403.138805	22.849203
105.617076	3420.063064	22.854221
105.544708	3432.967319	22.859239
105.531679	3436.192288	22.864256
105.730604	3432.642385	22.869274
105.477198	3443.675681	22.874291
105.445915	3429.967656	22.879309
105.700244	3445.238509	22.884327
106.275834	3453.373158	22.889344
106.333347	3454.080742	22.894362
106.151281	3461.384438	22.899379
106.506469	3467.677711	22.904397
106.510873	3470.701228	22.909415
106.483538	3465.236117	22.914432
106.642445	3462.387715	22.919450
106.562458	3487.793031	22.924467
106.838163	3488.738077	22.929485
106.762590	3496.587441	22.934503
106.987650	3488.921862	22.939520
107.327544	3491.701210	22.944538
107.393252	3510.997509	22.949555
107.220939	3520.463840	22.954573
107.194517	3524.802405	22.959591
107.501518	3525.957098	22.964608
107.566963	3528.391287	22.969626
107.581362	3549.034535	22.974643
107.466038	3551.105137	22.979661
107.473683	3557.367456	22.984679
107.492528	3577.667380	22.989696
107.919064	3587.578459	22.994714
107.776732	3598.605421	22.999731
108.424300	3610.369621	23.004749
108.474262	3620.600459	23.009767
109.054276	3623.965586	23.014784
109.120309	3609.048312	23.019802
109.020950	3619.851335	23.024819
109.166023	3616.231865	23.029837
109.614026	3606.730730	23.034855
109.473928	3608.777233	23.039872
109.644198	3609.813608	23.044890
109.751679	3631.668070	23.049907
109.925266	3633.112637	23.054925
110.183600	3638.649170	23.059943
109.853874	3646.558719	23.064960
110.244139	3635.039420	23.069978
110.383890	3637.408118	23.074995
110.683396	3637.300811	23.080013
110.737805	3635.201964	23.085031
110.633132	3637.913425	23.090048
110.622662	3627.671783	23.095066
110.368098	3638.050925	23.100083
110.639526	3635.894396	23.105101
110.690670	3639.222605	23.110119
110.795774	3643.261422	23.115136
111.304299	3642.277922	23.120154
111.018278	3661.478762	23.125171
111.014696	3665.414141	23.130189
111.130968	3671.552345	23.135207
110.995527	3674.371474	23.140224
110.936878	3667.604258	23.145242
110.882823	3688.238159	23.150259
110.872334	3690.811406	23.155277
111.331604	3711.394351	23.160295
111.502393	3725.872515	23.165312
111.709798	3727.864972	23.170330
111.566639	3742.378070	23.175347
111.951787	3749.965854	23.180365
112.233587	3758.151029	23.185383
112.009173	3762.801623	23.190400
112.632005	3784.738856	23.195418
112.177557	3795.414638	23.200435
112.506438	3792.360616	23.205453
112.877927	3796.512899	23.210471
112.765669	3800.485845	23.215488
113.590768	3814.840891	23.220506
113.364319	3820.494465	23.225523
113.699053	3819.763639	23.230541
113.781178	3818.665781	23.235559
113.810814	3813.825588	23.240576
114.084168	3813.716462	23.245594
113.907122	3822.192198	23.250611
113.919698	3818.745828	23.255629
114.226984	3806.861007	23.260647
114.057820	3820.336643	23.265664
114.288832	3829.240977	23.270682
114.333973	3845.979937	23.275699
114.192611	3840.346008	23.280717
114.325964	3843.942916	23.285735
114.197242	3856.716985	23.290752
114.799388	3867.974076	23.295770
114.403981	3882.844800	23.300787
114.635741	3886.300406	23.305805
114.939841	3904.178800	23.310823
114.797076	3924.484034	23.315840
115.341521	3912.728600	23.320858
115.427263	3925.010722	23.325875
115.385624	3938.178695	23.330893
115.744473	3934.161781	23.335911
115.709844	3937.668579	23.340928
116.145270	3923.434331	23.345946
115.919587	3939.588161	23.350963
116.051870	3963.828425	23.355981
116.280451	3963.153598	23.360999
116.304924	3962.779973	23.366016
116.441769	3970.199352	23.371034
116.443068	3973.451116	23.376051
116.610728	3988.363241	23.381069
117.031318	3996.771268	23.386087
116.708133	4001.301821	23.391104
116.957128	3997.350192	23.396122
116.905629	4009.154202	23.401139
117.021711	4022.779585	23.406157
117.734026	4035.273359	23.411175
117.478058	4037.054666	23.416192
117.648201	4036.537925	23.421210
117.415971	4034.318829	23.426227
117.320405	4036.971301	23.431245
117.520070	4052.779813	23.436263
117.388231	4060.843882	23.441280
118.151852	4077.757632	23.446298
118.002136	4088.772024	23.451315
118.649417	4088.085270	23.456333
119.200405	4090.088969	23.461351
118.959654	4087.353078	23.466368
119.184499	4085.152493	23.471386
119.050332	4082.514897	23.476403
118.851716	4088.182696	23.481421
118.901824	4091.964056	23.486439
119.030632	4114.280222	23.491456
119.040804	4110.961794	23.496474
119.239756	4128.333130	23.501491
119.079340	4133.342251	23.506509
119.542506	4143.580564	23.511527
119.738389	4146.104328	23.516544
119.985628	4140.183927	23.521562
120.468766	4155.490279	23.526579
120.473731	4164.535945	23.531597
120.741157	4163.674874	23.536615
120.622179	4161.678143	23.541632
121.189873	4157.240225	23.546650
121.261613	4159.575768	23.551667
121.072572	4161.280243	23.556685
121.120470	4160.420577	23.561703
121.045723	4166.848484	23.566720
121.277765	4160.621147	23.571738
121.174987	4161.250702	23.576755
121.263898	4169.217123	23.581773
121.378149	4179.066334	23.586791
121.497526	4193.458439	23.591808
121.453497	4189.308110	23.596826
121.388052	4200.503462	23.601843
121.643395	4225.143619	23.606861
121.581519	4237.804932	23.611879
121.722212	4245.793231	23.616896
121.986207	4265.477048	23.621914
122.237334	4270.773240	23.626931
122.238274	4275.847684	23.631949
122.590542	4287.737843	23.636967
122.665595	4305.512612	23.641984
122.809606	4299.364110	23.647002
123.144927	4300.970043	23.652019
123.389499	4315.082455	23.657037
123.654800	4332.950659	23.662055
123.546884	4334.970472	23.667072
123.477038	4337.808402	23.672090
123.881295	4334.865013	23.677107
123.666763	4337.626931	23.682125
124.114351	4332.966967	23.687143
123.603047	4332.561527	23.692160
123.588020	4345.365331	23.697178
124.092847	4364.748069	23.702195
123.577726	4371.243677	23.707213
124.195647	4381.988051	23.712231
124.385364	4398.338140	23.717248
124.200131	4394.266311	23.722266
124.469199	4405.951074	23.727283
124.661741	4411.786644	23.732301
124.890385	4426.219301	23.737319
125.042106	4430.290497	23.742336
125.899008	4431.557348	23.747354
126.522156	4435.353971	23.752371
126.048629	4427.888039	23.757389
126.070098	4417.523841	23.762407
125.820212	4419.501055	23.767424
126.010917	4441.548728	23.772442
126.136370	4440.026744	23.777459
126.589464	4438.224116	23.782477
126.938595	4436.659848	23.787495
126.821736	4441.196110	23.792512
126.831644	4447.389082	23.797530
127.173534	4436.814777	23.802547
126.950049	4438.909550	23.807565
127.110743	4438.177818	23.812583
127.163320	4439.501432	23.817600
127.372509	4449.690545	23.822618
127.399996	4466.492261	23.827635
127.293443	4475.393395	23.832653
127.519658	4470.334995	23.837671
127.370984	4483.594232	23.842688
127.442664	4499.930793	23.847706
127.779617	4494.761248	23.852723
127.603099	4505.612758	23.857741
127.975082	4512.584088	23.862759
127.902325	4535.494623	23.867776
127.960631	4542.044797	23.872794
128.149954	4556.280316	23.877811
128.451145	4573.970148	23.882829
128.954182	4560.442853	23.887847
128.926565	4572.021861	23.892864
129.243221	4579.228758	23.897882
130.165427	4570.615338	23.902899
129.715562	4573.478288	23.907917
130.015668	4570.917388	23.912935
130.247324	4569.288969	23.917952
130.118680	4567.701052	23.922970
130.460258	4559.048552	23.927987
130.030024	4572.446711	23.933005
130.537706	4565.474904	23.938023
130.372491	4569.587080	23.943040
130.648740	4572.643756	23.948058
130.699545	4560.988224	23.953075
130.504976	4565.618183	23.958093
130.670243	4568.834083	23.963111
130.441142	4592.856078	23.968128
130.884312	4608.665147	23.973146
130.922245	4601.168950	23.978163
130.639824	4610.071954	23.983181
131.201296	4617.829991	23.988199
131.507035	4633.911539	23.993216
131.159186	4634.371250	23.998234
131.869347	4646.384634	24.003251
131.693975	4663.805765	24.008269
131.796204	4667.746095	24.013287
131.879370	4670.678362	24.018304
131.908734	4684.476711	24.023322
132.143992	4694.018796	24.028339
131.894836	4710.382220	24.033357
132.508154	4718.715851	24.038375
133.144231	4719.264447	24.043392
133.253353	4719.795473	24.048410
133.950093	4715.871668	24.053427
133.828030	4720.934260	24.058445
133.710246	4717.114645	24.063463
134.216300	4716.941996	24.068480
133.989510	4722.431329	24.073498
134.392727	4718.065564	24.078515
133.962738	4716.850650	24.083533
134.102849	4717.104627	24.088551
134.392710	4719.847091	24.093568
134.363916	4719.621993	24.098586
134.581246	4706.940649	24.103603
134.536000	4717.895035	24.108621
134.430024	4730.871484	24.113639
134.759986	4750.063345	24.118656
134.546221	4746.365722	24.123674
134.806928	4752.040868	24.128691
134.401353	4779.052583	24.133709
134.671749	4776.121035	24.138727
134.871828	4806.841968	24.143744
134.733315	4817.005071	24.148762
135.405102	4838.589603	24.153779
135.334532	4855.145466	24.158797
135.570215	4865.328730	24.163815
135.781836	4871.210822	24.168832
135.751337	4881.720920	24.173850
136.186318	4889.497625	24.178867
136.216616	4908.277123	24.183885
136.266274	4912.269059	24.188903
136.469352	4912.393309	24.193920
136.911644	4923.962119	24.198938
137.234169	4931.411556	24.203955
137.219616	4929.429907	24.208973
137.315387	4933.408430	24.213991
137.491396	4953.448454	24.219008
137.593362	4963.867372	24.224026
137.892948	4961.155269	24.229043
137.965220	4955.501646	24.234061
138.193354	4954.751242	24.239079
138.319152	4948.562291	24.244096
138.433502	4954.605230	24.249114
138.313616	4960.359874	24.254131
138.282330	4980.374032	24.259149
138.426336	4987.041237	24.264167
139.167239	4971.226420	24.269184
139.156872	4980.005801	24.274202
139.377987	4970.549842	24.279219
139.273803	4981.286092	24.284237
139.534325	4997.163882	24.289255
139.397728	5000.582062	24.294272
139.545225	5013.310497	24.299290
139.580330	5013.298136	24.304307
139.396645	5024.600981	24.309325
139.728957	5033.373631	24.314343
139.922324	5039.105321	24.319360
140.241234	5054.277656	24.324378
140.311265	5065.129814	24.329395
140.412301	5075.201606	24.334413
140.674020	5075.362277	24.339431
140.722937	5071.208386	24.344448
140.547390	5095.115625	24.349466
140.957811	5099.680619	24.354483
141.119425	5101.731513	24.359501
141.310879	5128.268119	24.364519
141.827972	5127.711559	24.369536
141.906619	5124.710424	24.374554
141.947120	5112.686052	24.379571
142.096344	5125.200036	24.384589
142.224945	5135.070224	24.389607
142.324335	5144.921797	24.394624
142.216090	5153.336035	24.399642
142.708704	5154.222736	24.404659
142.682197	5149.252343	24.409677
142.448935	5161.493229	24.414695
142.827387	5180.933292	24.419712
142.353379	5192.988625	24.424730
143.005483	5204.959616	24.429747
143.152391	5223.061793	24.434765
142.902164	5226.796451	24.439783
143.206343	5249.271617	24.444800
142.941796	5267.509756	24.449818
143.134334	5273.064447	24.454835
143.324210	5284.891040	24.459853
144.171698	5305.039308	24.464871
144.635483	5307.094353	24.469888
144.783650	5318.496476	24.474906
144.649436	5312.222780	24.479923
145.119036	5312.981894	24.484941
145.291741	5307.507848	24.489959
145.308820	5319.302650	24.494976
145.238026	5334.115140	24.499994
145.530201	5340.733464	24.505011
145.562464	5342.312693	24.510029
145.706781	5343.243360	24.515047
146.064909	5333.380888	24.520064
146.026957	5334.080506	24.525082
146.080353	5338.168793	24.530099
146.201538	5362.638375	24.535117
146.145502	5370.915387	24.540135
146.467781	5373.328675	24.545152
146.591819	5381.486602	24.550170
146.639113	5382.192088	24.555187
146.964062	5405.658751	24.560205
146.917272	5403.603013	24.565223
147.422419	5402.308076	24.570240
147.617378	5409.477928	24.575258
147.549314	5420.631266	24.580275
147.658215	5432.222156	24.585293
147.549373	5446.651372	24.590311
147.927015	5431.209509	24.595328
147.855297	5450.296214	24.600346
147.929593	5462.364091	24.605363
148.280159	5471.801022	24.610381
148.476066	5474.978772	24.615399
148.764164	5476.594500	24.620416
148.363107	5502.146303	24.625434
148.792278	5502.311357	24.630451
148.910063	5495.326433	24.635469
149.221538	5521.791134	24.640487
149.626478	5525.262312	24.645504
149.240231	5533.487316	24.650522
149.272617	5535.358774	24.655539
149.720812	5550.185682	24.660557
149.720093	5552.819782	24.665575
150.027334	5567.158086	24.670592
149.823317	5593.263871	24.675610
150.254202	5587.960508	24.680627
150.866998	5608.218712	24.685645
150.657885	5630.693402	24.690663
150.764223	5624.269644	24.695680
150.774478	5639.371784	24.700698
150.982468	5645.508423	24.705715
151.061127	5663.277792	24.710733
151.175398	5669.293448	24.715751
151.249061	5673.530372	24.720768
151.376766	5698.679131	24.725786
151.363988	5702.799336	24.730803
151.569364	5721.210284	24.735821
151.923232	5713.824818	24.740839
152.180024	5731.069842	24.745856
152.551642	5749.869016	24.750874
152.714541	5755.905513	24.755891
152.457637	5756.786831	24.760909
152.685726	5785.549007	24.765927
153.122713	5785.718239	24.770944
153.076568	5791.954427	24.775962
153.424359	5800.976126	24.780979
153.490946	5811.939662	24.785997
153.539051	5828.365127	24.791015
154.088712	5817.687339	24.796032
154.624522	5819.524518	24.801050
154.434159	5816.460667	24.806067
154.671410	5813.120285	24.811085
154.803935	5821.697615	24.816103
154.621838	5825.613719	24.821120
154.900416	5844.387994	24.826138
154.738066	5844.761583	24.831155
154.946026	5838.961505	24.836173
155.086684	5860.475430	24.841191
155.125091	5876.887641	24.846208
155.041795	5882.178690	24.851226
154.906896	5894.356800	24.856243
155.204845	5906.961696	24.861261
154.790453	5929.193937	24.866279
154.960094	5940.207638	24.871296
154.979954	5972.890806	24.876314
155.568743	5992.141415	24.881331
155.806952	6008.135108	24.886349
155.775159	6041.065158	24.891367
156.508410	6049.109541	24.896384
157.092502	6072.766714	24.901402
157.200305	6070.684389	24.906419
157.735329	6065.734817	24.911437
157.938521	6064.606600	24.916455
158.358185	6060.668534	24.921472
158.786035	6065.111878	24.926490
158.342769	6063.774671	24.931507
158.748204	6054.058039	24.936525
158.516086	6064.053658	24.941543
158.583153	6068.857393	24.946560
158.986374	6080.881956	24.951578
159.105932	6081.453778	24.956595
159.018438	6090.865346	24.961613
159.432602	6088.069610	24.966631
159.159958	6091.200986	24.971648
159.227856	6111.212952	24.976666
159.423035	6128.622574	24.981683
159.668516	6130.729333	24.986701
159.611631	6153.396070	24.991719
159.692598	6154.566084	24.996736
159.730550	6168.152351	25.001754
159.732700	6187.222547	25.006771
160.296391	6199.602522	25.011789
160.123030	6224.965991	25.016807
160.317255	6224.797954	25.021824
160.462236	6246.803983	25.026842
160.799558	6259.561529	25.031859
161.049434	6261.246909	25.036877
161.058485	6294.003483	25.041895
161.317147	6303.321176	25.046912
161.749943	6310.994192	25.051930
162.269068	6323.121167	25.056947
162.531078	6318.894975	25.061965
162.323908	6322.577605	25.066983
162.836520	6324.911149	25.072000
162.962905	6316.422205	25.077018
162.839442	6312.542524	25.082035
162.867265	6312.220260	25.087053
162.641426	6333.317139	25.092071
163.255430	6346.700041	25.097088
163.131884	6350.778746	25.102106
162.991487	6365.521414	25.107123
163.360564	6383.890887	25.112141
163.181040	6384.693591	25.117159
163.386896	6401.441566	25.122176
163.511221	6417.019579	25.127194
163.422072	6457.393322	25.132211
163.793169	6459.274570	25.137229
164.146027	6483.356406	25.142247
164.237194	6491.457519	25.147264
164.521439	6510.942930	25.152282
164.746943	6527.661673	25.157299
165.338620	6535.395789	25.162317
164.967375	6554.249999	25.167335
164.961791	6558.179347	25.172352
165.491234	6582.508344	25.177370
165.580386	6590.947004	25.182387
166.104526	6596.452405	25.187405
166.185836	6621.889431	25.192423
166.292696	6624.762069	25.197440
166.366544	6636.083347	25.202458
166.526168	6651.260881	25.207475
166.703325	6655.860015	25.212493
166.741502	6668.309960	25.217511
167.202073	6683.003465	25.222528
167.233222	6693.471891	25.227546
167.263245	6709.961230	25.232563
167.549116	6715.640646	25.237581
167.726742	6735.679485	25.242599
167.565120	6752.358481	25.247616
168.162221	6751.889780	25.252634
168.247976	6773.950801	25.257651
168.504129	6774.457482	25.262669
168.869222	6779.056733	25.267687
169.193664	6789.932625	25.272704
169.591367	6794.528653	25.277722
169.976231	6796.357166	25.282739
170.266368	6793.820472	25.287757
170.190109	6801.710181	25.292775
170.517435	6789.033540	25.297792
170.677450	6789.554339	25.302810
170.654040	6793.633321	25.307827
170.636870	6789.216177	25.312845
170.486992	6803.765512	25.317863
170.684853	6795.069488	25.322880
170.907552	6801.342697	25.327898
171.196677	6815.051096	25.332915
171.690696	6824.970764	25.337933
171.287465	6834.070590	25.342951
171.161541	6840.465808	25.347968
171.375973	6829.846394	25.352986
171.376947	6847.182170	25.358003
171.960051	6856.750217	25.363021
171.714429	6864.635117	25.368039
171.783463	6885.652239	25.373056
172.162867	6891.763127	25.378074
172.227828	6910.958912	25.383091
172.490874	6924.853847	25.388109
172.890445	6924.233882	25.393127
172.742321	6941.079340	25.398144
173.001433	6964.772280	25.403162
172.663895	6975.378928	25.408179
173.085462	6989.878525	25.413197
172.950371	7012.878927	25.418215
173.320931	7029.516612	25.423232
173.909171	7042.823379	25.428250
173.825556	7063.774734	25.433267
174.242227	7063.151833	25.438285
174.467863	7092.802227	25.443303
174.693891	7104.750804	25.448320
174.988132	7097.927148	25.453338
175.239755	7123.219974	25.458355
175.423199	7125.663636	25.463373
175.294302	7118.491054	25.468391
175.668307	7144.945367	25.473408
175.796142	7153.300492	25.478426
175.961987	7166.421384	25.483443
176.243860	7181.379161	25.488461
176.471259	7192.052964	25.493479
176.380146	7194.464137	25.498496
176.849902	7197.040704	25.503514
176.568778	7222.410831	25.508531
177.023783	7230.710701	25.513549
177.123146	7243.674471	25.518567
177.405976	7258.943324	25.523584
177.714146	7258.202732	25.528602
177.199586	7272.235207	25.533619
177.591796	7290.300830	25.538637
177.896932	7297.674798	25.543655
178.017971	7325.284319	25.548672
178.240194	7323.658033	25.553690
178.357845	7341.371379	25.558707
178.525119	7357.447909	25.563725
178.760875	7370.174913	25.568743
178.976721	7393.563158	25.573760
179.548835	7397.117960	25.578778
179.485908	7404.786678	25.583795
179.638150	7428.451357	25.588813
179.658360	7433.751958	25.593831
179.689206	7445.002402	25.598848
180.599498	7447.666563	25.603866
180.246699	7457.868863	25.608883
180.499354	7462.583696	25.613901
180.280474	7483.016006	25.618919
180.732577	7501.964945	25.623936
180.794889	7500.395989	25.628954
180.877977	7527.629502	25.633971
181.182289	7529.706670	25.638989
181.446909	7538.519096	25.644007
182.051416	7541.295563	25.649024
183.127696	7526.727686	25.654042
183.174799	7533.014740	25.659059
183.183942	7530.140087	25.664077
183.557681	7527.445572	25.669095
183.304576	7532.092719	25.674112
183.799976	7527.344081	25.679130
183.534066	7527.727580	25.684148
183.508013	7526.855202	25.689165
183.783602	7526.888272	25.694183
183.797916	7531.529754	25.699200
184.045222	7541.959318	25.704218
183.817836	7561.202057	25.709236
184.001475	7560.645871	25.714253
184.525132	7583.281287	25.719271
184.188446	7601.198061	25.724288
184.293611	7601.699143	25.729306
184.243314	7626.047181	25.734324
184.543571	7647.068993	25.739341
184.756062	7658.282935	25.744359
184.825171	7679.836781	25.749376
185.074126	7708.236457	25.754394
185.263432	7719.723841	25.759412
185.491890	7740.164875	25.764429
186.037146	7756.945110	25.769447
185.748616	7779.443513	25.774464
186.255667	7783.598040	25.779482
186.140124	7815.820534	25.784500
186.401749	7826.944241	25.789517
186.611092	7841.653519	25.794535
186.913342	7852.946746	25.799552
187.135540	7875.842231	25.804570
187.711948	7887.164115	25.809588
188.199345	7899.519104	25.814605
188.272907	7904.574374	25.819623
188.575815	7911.518082	25.824640
188.571939	7912.700406	25.829658
188.692655	7928.179670	25.834676
189.096381	7935.074593	25.839693
189.556017	7922.179007	25.844711
189.423046	7933.154571	25.849728
189.469837	7946.473766	25.854746
189.613082	7958.200043	25.859764
189.744953	7959.497754	25.864781
190.088765	7979.304045	25.869799
190.116232	7989.921268	25.874816
190.555404	7988.208096	25.879834
190.143524	7999.310296	25.884852
190.700269	8018.694898	25.889869
190.821120	8031.093914	25.894887
191.220500	8035.946843	25.899904
191.136291	8027.085800	25.904922
191.244200	8052.218017	25.909940
191.029281	8061.672278	25.914957
191.670311	8074.882625	25.919975
191.345980	8101.082440	25.924992
191.641895	8105.837317	25.930010
192.286864	8137.069010	25.935028
192.175252	8139.185257	25.940045
192.987715	8144.344771	25.945063
192.894962	8165.696186	25.950080
193.181572	8164.886773	25.955098
193.165799	8176.579018	25.960116
193.366490	8187.300606	25.965133
193.843813	8191.276776	25.970151
194.053315	8216.472979	25.975168
194.145341	8225.858964	25.980186
194.209944	8226.263027	25.985204
194.080755	8235.980793	25.990221
194.789327	8248.892153	25.995239
194.679284	8263.979573	26.000256
194.913895	8274.960111	26.005274
195.207450	8295.293004	26.010292
195.228814	8298.049034	26.015309
195.816496	8309.443341	26.020327
195.710842	8323.635887	26.025344
195.957936	8327.538111	26.030362
196.078747	8347.518588	26.035380
196.169105	8361.831981	26.040397
196.495904	8364.419855	26.045415
196.661987	8387.926798	26.050432
197.705823	8365.730505	26.055450
198.321485	8362.887241	26.060468
198.509961	8353.747654	26.065485
198.790644	8353.137781	26.070503
199.063365	8350.678675	26.075520
199.177854	8352.578932	26.080538
199.237319	8352.935822	26.085556
198.917548	8355.733794	26.090573
199.090419	8342.734193	26.095591
199.427855	8349.363346	26.100608
199.355202	8344.734695	26.105626
199.165837	8344.558340	26.110644
199.523785	8359.285950	26.115661
199.973736	8367.024775	26.120679
199.941862	8373.687307	26.125696
199.868018	8371.022109	26.130714
200.322208	8382.413354	26.135732
199.842237	8403.580144	26.140749
200.150490	8416.209680	26.145767
200.442432	8436.123118	26.150784
200.405972	8446.697240	26.155802
200.711968	8468.503821	26.160820
200.436427	8483.119544	26.165837
200.937744	8496.028816	26.170855
201.082637	8530.060284	26.175872
201.731058	8532.611174	26.180890
202.091020	8535.022432	26.185908
202.527228	8562.472908	26.190925
202.846707	8574.092217	26.195943
202.952458	8578.362227	26.200960
202.737987	8576.720863	26.205978
202.697349	8600.659833	26.210996
202.719055	8611.533712	26.216013
203.261520	8617.117826	26.221031
203.292186	8629.289322	26.226048
204.009625	8649.614606	26.231066
204.082960	8668.618823	26.236084
203.809876	8677.104130	26.241101
204.387900	8688.624843	26.246119
204.873570	8710.227629	26.251136
204.828770	8705.610644	26.256154
204.950344	8725.725392	26.261172
204.944707	8737.091716	26.266189
205.621955	8745.881348	26.271207
205.716176	8752.111168	26.276224
205.740700	8761.754843	26.281242
206.555042	8776.801676	26.286260
206.514138	8789.308577	26.291277
206.897007	8791.729341	26.296295
206.786072	8801.601099	26.301312
207.131247	8814.438914	26.306330
207.220394	8821.800977	26.311348
206.954788	8825.665940	26.316365
207.866555	8848.706961	26.321383
207.604455	8861.650485	26.326400
207.558404	8876.039716	26.331418
208.470007	8883.022895	26.336436
208.281244	8889.115344	26.341453
208.234266	8905.069428	26.346471
208.810422	8931.117806	26.351488
208.865420	8938.088699	26.356506
209.178515	8946.605238	26.361524
208.876293	8961.805824	26.366541
209.595654	8973.339544	26.371559
209.518602	8986.883306	26.376576
209.961823	9005.339198	26.381594
210.296726	9017.279205	26.386612
210.372704	9045.075881	26.391629
210.407664	9053.781968	26.396647
210.602139	9070.916005	26.401664
210.760323	9085.623374	26.406682
211.059927	9102.433735	26.411700
211.318722	9130.700298	26.416717
211.723125	9125.459418	26.421735
212.014821	9149.615622	26.426752
212.319367	9152.544645	26.431770
212.801745	9143.028061	26.436788
212.775491	9147.090006	26.441805
213.675475	9161.485929	26.446823
214.031630	9163.147104	26.451840
214.182873	9165.988956	26.456858
214.397179	9158.199613	26.461876
213.922088	9153.842193	26.466893
214.040709	9166.928695	26.471911
213.829813	9179.039590	26.476928
213.886828	9180.397505	26.481946
214.619526	9197.664748	26.486964
214.505926	9208.367619	26.491981
214.625271	9218.598818	26.496999
214.702592	9241.165753	26.502016
214.750148	9254.297597	26.507034
215.014665	9267.827165	26.512052
215.084504	9295.335388	26.517069
215.292969	9315.747974	26.522087
215.446975	9339.833521	26.527104
215.604474	9359.424482	26.532122
215.584930	9384.984801	26.537140
215.394405	9409.567566	26.542157
215.886158	9442.474718	26.547175
216.181105	9458.678008	26.552192
216.484807	9490.084283	26.557210
217.475888	9499.706112	26.562228
217.939528	9513.646117	26.567245
218.402283	9519.491607	26.572263
218.733152	9530.053897	26.577280
218.733648	9532.606502	26.582298
219.211144	9530.354788	26.587316
219.476606	9551.419721	26.592333
219.861421	9562.292665	26.597351
219.767565	9558.749061	26.602368
219.748693	9563.299908	26.607386
220.059341	9563.720921	26.612404
220.341154	9587.521777	26.617421
220.325427	9603.780042	26.622439
220.747184	9604.582257	26.627456
220.836628	9624.460964	26.632474
220.982911	9634.665748	26.637492
221.045308	9643.547087	26.642509
221.108176	9660.830371	26.647527
221.389259	9675.663757	26.652544
221.190083	9700.550995	26.657562
221.782099	9714.473897	26.662580
221.785851	9742.161239	26.667597
221.651856	9758.009744	26.672615
222.179904	9778.654926	26.677632
222.493129	9801.568272	26.682650
222.327756	9824.015313	26.687668
222.623691	9848.015832	26.692685
223.003987	9862.069700	26.697703
223.218643	9883.035044	26.702720
222.921895	9911.015280	26.707738
223.688250	9917.491196	26.712756
223.797808	9948.479385	26.717773
223.624079	9974.788780	26.722791
224.277426	9984.883231	26.727808
224.404044	10021.371346	26.732826
224.728558	10040.780074	26.737844
224.885267	10063.982204	26.742861
225.649766	10072.165107	26.747879
225.885744	10093.617146	26.752896
226.042169	10099.817914	26.757914
226.506436	10126.438938	26.762932
226.889954	10138.662969	26.767949
227.021767	10144.091094	26.772967
227.590017	10150.393054	26.777984
228.046777	10146.650936	26.783002
228.346515	10139.314498	26.788020
228.827261	10141.937734	26.793037
228.921555	10120.406872	26.798055
230.024917	10107.481946	26.803072
230.090388	10110.751532	26.808090
230.244543	10090.809903	26.813108
230.456095	10078.107201	26.818125
230.445227	10067.650349	26.823143
230.547714	10062.497166	26.828160
230.380742	10066.884442	26.833178
230.781591	10070.934865	26.838196
230.665934	10071.463635	26.843213
230.485248	10064.482197	26.848231
230.799834	10083.598002	26.853248
230.593878	10097.150605	26.858266
230.974257	10106.626929	26.863284
231.075811	10127.998053	26.868301
231.133829	10144.159125	26.873319
231.317052	10166.384577	26.878336
231.100315	10183.475245	26.883354
231.294015	10202.140740	26.888372
231.695700	10240.276213	26.893389
232.000748	10254.013973	26.898407
232.477589	10271.365622	26.903424
232.131308	10295.361851	26.908442
232.500377	10321.499975	26.913460
232.556858	10346.229342	26.918477
232.643968	10374.453443	26.923495
233.364155	10398.646798	26.928512
233.683532	10421.548937	26.933530
234.101121	10443.112135	26.938548
234.179794	10460.929351	26.943565
234.106947	10485.999421	26.948583
234.616550	10504.423588	26.953600
234.858825	10529.630389	26.958618
235.558757	10551.099635	26.963636
235.507758	10568.017318	26.968653
235.654851	10580.375185	26.973671
235.852392	10597.069072	26.978688
236.116679	10627.953243	26.983706
236.347164	10638.238778	26.988724
236.716252	10664.363268	26.993741
236.752023	10676.808053	26.998759
237.226173	10688.181754	27.003776
236.983440	10709.300632	27.008794
237.072929	10718.568733	27.013812
237.771388	10749.003655	27.018829
238.032675	10768.123099	27.023847
238.541759	10786.711568	27.028864
238.488122	10798.829805	27.033882
239.133625	10813.379570	27.038900
239.547068	10838.368404	27.043917
239.729910	10839.432263	27.048935
240.062915	10849.222865	27.053952
240.006464	10868.481989	27.058970
240.435140	10867.674103	27.063988
240.393431	10879.312861	27.069005
240.241207	10900.526785	27.074023
240.946006	10917.857388	27.079040
241.080640	10929.105075	27.084058
241.355662	10947.097186	27.089076
241.746908	10971.656658	27.094093
241.722521	10971.444897	27.099111
242.806065	10974.918368	27.104128
242.768112	10984.384966	27.109146
243.051024	10991.866090	27.114164
243.262952	11011.567910	27.119181
243.278494	11023.474317	27.124199
243.483124	11020.804286	27.129216
243.664302	11041.512113	27.134234
243.670415	11053.629753	27.139252
243.851054	11076.113765	27.144269
243.868678	11095.262753	27.149287
244.302195	11107.289838	27.154304
244.194637	11139.521511	27.159322
244.712481	11150.624870	27.164340
244.817352	11184.900433	27.169357
245.138116	11212.293248	27.174375
245.455816	11230.892968	27.179392
245.508718	11257.375185	27.184410
245.560928	11278.346536	27.189428
245.789602	11297.153855	27.194445
246.231225	11326.338467	27.199463
246.576827	11348.573948	27.204480
247.069263	11369.714229	27.209498
247.230442	11386.657853	27.214516
247.624884	11404.158795	27.219533
247.815010	11429.390111	27.224551
248.438554	11443.356380	27.229568
248.703690	11456.351850	27.234586
248.890339	11471.817686	27.239604
249.530815	11478.051057	27.244621
249.285923	11483.380301	27.249639
249.722757	11498.242242	27.254656
249.792871	11510.804701	27.259674
250.029532	11529.357191	27.264692
250.166387	11539.011628	27.269709
250.195326	11552.536206	27.274727
250.442125	11558.287078	27.279744
250.754073	11568.343333	27.284762
250.743054	11598.422365	27.289780
251.302845	11613.343709	27.294797
250.944850	11633.277926	27.299815
251.441767	11639.170343	27.304832
251.639279	11668.255573	27.309850
251.740569	11703.804644	27.314868
252.566036	11713.536574	27.319885
252.624016	11747.525071	27.324903
252.593561	11755.704835	27.329920
252.921057	11778.040140	27.334938
253.479422	11806.171760	27.339956
254.012714	11811.030466	27.344973
254.120178	11837.228474	27.349991
254.596285	11843.953501	27.355008
255.105513	11856.324337	27.360026
255.759109	11862.070205	27.365044
256.147239	11859.251964	27.370061
256.348633	11861.348135	27.375079
256.668412	11856.355717	27.380096
256.758954	11854.448972	27.385114
256.578645	11870.045853	27.390132
256.986110	11889.283398	27.395149
257.426056	11892.262214	27.400167
257.719487	11894.720851	27.405184
257.831876	11899.864487	27.410202
257.951258	11916.327269	27.415220
257.908249	11921.451844	27.420237
258.174164	11937.129903	27.425255
258.232146	11948.883142	27.430272
258.214015	11974.381093	27.435290
258.324850	11997.875947	27.440308
258.708406	12017.354141	27.445325
258.594590	12047.858227	27.450343
259.004207	12064.001914	27.455360
259.760571	12083.629047	27.460378
259.180834	12106.775926	27.465396
260.309156	12119.042423	27.470413
260.639836	12146.494996	27.475431
260.913494	12164.205004	27.480448
261.292263	12176.387259	27.485466
261.393056	12193.345223	27.490484
261.626421	12201.401189	27.495501
261.730518	12228.229233	27.500519
262.009026	12235.234151	27.505536
262.330577	12267.087170	27.510554
262.097963	12281.460955	27.515572
262.704042	12294.936079	27.520589
262.726227	12321.898095	27.525607
262.751830	12343.360789	27.530624
263.136973	12374.687755	27.535642
263.095611	12396.671057	27.540660
263.780173	12416.016180	27.545677
263.753249	12443.639293	27.550695
264.390442	12459.731756	27.555712
264.910435	12465.916816	27.560730
265.273775	12485.813535	27.565748
265.484169	12493.966569	27.570765
265.900228	12509.015815	27.575783
266.454809	12525.990906	27.580800
266.851303	12525.574597	27.585818
266.874479	12541.597444	27.590836
267.438389	12556.761661	27.595853
267.815391	12576.443381	27.600871
267.822554	12569.215900	27.605888
267.996105	12579.925348	27.610906
267.886634	12596.959172	27.615924
268.414881	12589.853559	27.620941
268.545996	12623.267111	27.625959
268.907182	12631.722189	27.630976
268.789454	12644.308259	27.635994
268.978815	12657.779460	27.641012
269.335459	12681.116533	27.646029
269.607172	12710.274430	27.651047
269.751952	12727.464970	27.656064
270.122770	12750.765039	27.661082
270.196988	12765.762790	27.666100
270.759841	12788.624947	27.671117
270.574281	12812.636714	27.676135
270.638456	12830.533076	27.681152
271.435424	12860.869954	27.686170
271.514071	12878.117694	27.691188
272.210868	12900.575638	27.696205
272.507110	12923.931290	27.701223
272.725510	12939.966770	27.706240
272.816248	12954.093436	27.711258
273.291522	12971.440357	27.716276
273.576510	12974.735937	27.721293
273.955963	13001.924682	27.726311
274.366576	13013.419655	27.731328
274.395858	13039.391843	27.736346
274.506584	13054.591645	27.741364
274.768871	13076.766531	27.746381
274.952621	13096.352760	27.751399
275.713631	13111.931324	27.756416
276.058600	13113.464022	27.761434
276.873379	13127.253961	27.766452
277.280944	13120.658977	27.771469
277.375611	13124.196831	27.776487
277.700828	13133.903460	27.781504
278.190965	13139.632097	27.786522
278.165928	13151.115152	27.791540
278.550303	13140.785602	27.796557
278.637671	13147.223177	27.801575
279.234513	13130.789195	27.806592
280.247563	13137.608710	27.811610
280.164326	13130.242019	27.816628
279.957207	13120.671100	27.821645
280.246469	13117.827040	27.826663
280.355361	13115.333846	27.831680
280.719667	13128.698221	27.836698
280.501211	13147.502351	27.841716
281.080256	13144.603890	27.846733
281.101278	13159.735632	27.851751
281.230154	13161.201349	27.856768
281.714583	13187.431472	27.861786
281.036655	13198.611948	27.866804
281.236104	13213.780930	27.871821
281.228598	13232.139209	27.876839
281.609519	13263.050928	27.881856
282.023164	13292.057866	27.886874
282.074611	13325.407697	27.891892
282.334223	13349.734824	27.896909
282.830130	13383.858127	27.901927
282.863956	13409.188635	27.906944
283.458505	13432.249581	27.911962
283.648274	13468.007972	27.916980
284.180726	13494.283943	27.921997
284.496801	13521.222772	27.927015
284.865204	13542.473817	27.932032
285.152775	13567.324483	27.937050
285.214225	13590.480177	27.942068
285.864896	13594.756619	27.947085
286.653009	13612.704704	27.952103
287.291246	13627.828808	27.957120
287.823501	13620.022258	27.962138
288.028106	13635.390917	27.967156
288.416471	13646.568614	27.972173
288.435981	13658.233527	27.977191
288.435730	13660.320362	27.982208
288.761066	13661.240200	27.987226
288.666180	13682.395878	27.992244
289.086524	13686.562088	27.997261
289.174301	13715.428607	28.002279
289.398864	13730.321085	28.007296
290.139747	13745.134538	28.012314
290.378659	13760.527381	28.017332
290.585451	13782.986987	28.022349
290.493789	13808.536639	28.027367
290.495735	13820.895040	28.032384
291.192175	13849.134181	28.037402
291.218630	13867.876663	28.042420
291.490814	13883.419960	28.047437
291.726302	13905.922101	28.052455
291.748471	13936.598676	28.057472
292.268186	13950.534459	28.062490
292.524514	13991.063151	28.067508
292.697872	14010.904441	28.072525
293.230627	14032.446341	28.077543
293.826745	14059.106352	28.082560
294.210656	14065.212897	28.087578
294.541110	14091.035824	28.092596
294.998522	14101.301987	28.097613
295.579840	14105.275213	28.102631
295.684597	14126.501272	28.107648
296.269497	14126.331627	28.112666
296.673816	14121.684992	28.117684
296.915856	14112.353328	28.122701
297.330650	14112.638413	28.127719
297.565272	14133.426105	28.132736
298.177623	14135.195216	28.137754
298.270148	14139.116674	28.142772
298.378508	14128.165507	28.147789
298.866418	14121.999271	28.152807
298.999158	14128.990583	28.157824
299.138012	14146.401140	28.162842
299.453134	14156.907666	28.167860
299.542323	14155.804755	28.172877
299.719451	14167.865436	28.177895
299.732086	14191.870461	28.182912
300.138522	14201.469230	28.187930
300.508562	14227.813618	28.192948
300.669542	14229.783047	28.197965
300.830535	14248.372077	28.202983
300.588744	14281.053771	28.208000
300.837426	14298.466155	28.213018
301.133980	14327.190779	28.218036
301.277637	14361.967569	28.223053
301.849638	14385.851783	28.228071
302.285169	14413.458835	28.233088
303.104744	14427.215955	28.238106
303.548297	14463.316032	28.243124
303.738307	14463.226679	28.248141
304.086612	14478.353976	28.253159
304.062593	14503.011991	28.258176
304.582345	14526.068381	28.263194
304.568403	14545.379698	28.268212
305.814902	14551.707425	28.273229
306.226726	14552.845777	28.278247
306.342016	14569.485307	28.283264
306.754579	14572.226577	28.288282
306.814756	14591.405450	28.293300
306.934348	14603.607140	28.298317
307.076745	14620.940354	28.303335
307.282750	14642.064605	28.308352
307.410060	14652.814856	28.313370
307.781266	14676.298861	28.318388
307.871044	14698.792380	28.323405
308.262623	14725.171701	28.328423
308.016620	14754.139803	28.333440
308.489247	14779.011022	28.338458
308.587970	14814.193683	28.343476
308.979689	14842.765758	28.348493
309.333374	14883.201141	28.353511
309.226495	14907.791994	28.358528
309.858455	14929.359048	28.363546
310.279410	14960.363244	28.368564
310.540618	14991.303453	28.373581
311.031438	15015.185154	28.378599
311.168150	15041.457338	28.383616
311.591228	15060.128464	28.388634
311.843119	15098.148024	28.393652
312.311624	15130.403849	28.398669
312.937099	15144.852156	28.403687
313.329551	15158.087255	28.408704
313.817811	15183.940015	28.413722
313.977076	15194.606327	28.418740
313.924850	15220.876499	28.423757
314.311223	15242.366255	28.428775
314.651789	15263.652665	28.433792
315.095546	15279.328656	28.438810
315.391213	15308.638373	28.443828
315.350624	15332.318416	28.448845
315.715938	15357.877257	28.453863
316.322894	15381.842044	28.458880
316.390229	15400.103205	28.463898
317.046137	15427.833390	28.468916
317.287831	15452.672691	28.473933
317.356688	15473.588211	28.478951
317.549671	15498.303517	28.483968
318.135012	15521.424143	28.488986
318.464237	15549.823718	28.494004
318.616452	15574.380609	28.499021
319.109388	15599.413520	28.504039
319.626619	15623.963095	28.509056
320.191485	15645.634014	28.514074
320.262742	15667.876653	28.519092
320.431446	15697.377486	28.524109
321.056902	15706.460385	28.529127
321.639948	15747.161226	28.534144
321.743693	15747.384585	28.539162
322.538615	15769.676731	28.544180
322.278363	15778.116986	28.549197
322.715288	15801.296544	28.554215
322.575971	15826.056680	28.559232
322.847177	15851.961872	28.564250
322.999096	15877.134044	28.569268
323.660366	15907.022163	28.574285
323.884893	15930.523628	28.579303
324.029284	15957.500585	28.584320
324.177334	15989.976949	28.589338
324.356035	16020.821295	28.594356
324.530845	16054.199618	28.599373
324.842416	16080.563282	28.604391
325.054924	16127.238442	28.609408
325.637542	16161.407797	28.614426
326.511804	16190.422856	28.619444
326.883193	16213.216968	28.624461
327.459659	16232.872026	28.629479
327.484656	16264.398950	28.634496
327.637501	16290.094955	28.639514
328.014786	16312.760504	28.644532
327.942014	16337.189981	28.649549
328.509490	16362.791388	28.654567
328.488850	16399.131304	28.659584
328.832324	16426.620341	28.664602
329.431546	16457.897879	28.669620
329.473666	16486.685615	28.674637
329.888836	16511.170445	28.679655
330.153384	16545.423478	28.684672
330.350248	16578.524771	28.689690
330.727386	16609.426054	28.694708
330.743980	16648.403819	28.699725
331.309530	16683.020150	28.704743
331.725661	16731.020998	28.709760
332.198692	16756.347554	28.714778
332.897942	16781.561284	28.719796
333.410734	16802.181684	28.724813
333.747358	16823.421898	28.729831
333.646722	16852.296213	28.734848
334.063000	16880.560175	28.739866
334.623569	16913.457916	28.744884
334.949624	16938.392175	28.749901
335.976297	16960.294651	28.754919
335.946339	16989.467654	28.759936
336.302667	17009.668985	28.764954
336.575757	17030.515197	28.769972
336.859650	17056.120556	28.774989
337.316323	17070.564795	28.780007
337.712676	17101.665486	28.785024
338.063415	17123.777037	28.790042
338.547312	17146.111727	28.795060
338.583871	17173.247862	28.800077
338.998519	17188.317391	28.805095
339.203623	17218.554053	28.810112
339.396159	17246.227959	28.815130
339.461578	17267.888850	28.820148
339.468848	17303.713585	28.825165
340.020186	17329.659770	28.830183
340.246444	17376.982434	28.835200
340.796080	17408.552450	28.840218
341.193526	17440.090277	28.845236
341.091428	17481.098807	28.850253
341.629849	17505.020072	28.855271
341.390258	17541.808313	28.860288
341.758828	17586.050292	28.865306
342.023339	17627.272239	28.870324
342.318963	17682.972622	28.875341
342.959450	17715.984370	28.880359
343.191189	17758.369439	28.885376
343.708774	17798.985607	28.890394
344.212648	17843.895607	28.895412
344.307880	17893.050491	28.900429
345.179434	17914.797929	28.905447
345.422385	17954.605470	28.910464
346.326305	17992.783166	28.915482
346.864514	18004.248715	28.920500
347.066631	18036.946814	28.925517
347.713104	18047.791586	28.930535
348.127434	18072.982002	28.935552
347.812590	18081.809570	28.940570
348.754497	18101.024247	28.945588
348.993537	18113.474479	28.950605
349.841207	18124.071982	28.955623
350.331783	18137.781379	28.960640
350.452686	18155.249657	28.965658
351.025488	18167.619079	28.970676
350.971515	18184.521409	28.975693
351.635882	18193.085042	28.980711
351.946594	18206.106397	28.985728
351.910362	18229.900158	28.990746
352.579926	18230.756544	28.995764
352.681796	18256.098534	29.000781
353.049694	18272.269634	29.005799
353.044697	18290.990951	29.010816
353.205989	18318.813876	29.015834
353.788647	18344.915506	29.020852
353.863657	18379.743974	29.025869
354.443678	18393.999524	29.030887
354.651168	18428.174745	29.035904
354.347015	18454.720203	29.040922
354.964526	18488.681804	29.045940
354.970217	18522.742023	29.050957
355.608259	18560.654412	29.055975
355.674242	18600.038168	29.060992
355.821047	18636.049944	29.066010
356.035621	18676.463177	29.071028
356.283452	18720.747759	29.076045
357.168841	18754.121624	29.081063
357.627219	18787.677526	29.086080
358.048650	18826.475871	29.091098
358.359815	18850.835323	29.096116
359.317139	18883.117111	29.101133
359.909139	18910.783636	29.106151
360.216743	18933.500944	29.111168
360.662517	18959.756275	29.116186
360.981855	18992.387266	29.121204
361.224953	19012.482708	29.126221
361.692168	19031.546465	29.131239
362.166215	19063.309139	29.136256
361.700386	19097.739859	29.141274
362.669029	19112.741406	29.146292
362.783542	19150.792149	29.151309
363.313878	19170.586284	29.156327
363.978602	19203.975212	29.161344
363.793395	19227.789604	29.166362
364.545683	19250.322337	29.171380
364.629001	19282.497683	29.176397
365.075357	19294.765052	29.181415
366.284182	19311.644448	29.186432
366.520759	19339.550758	29.191450
367.968736	19331.526303	29.196468
368.569201	19318.562263	29.201485
368.626391	19319.255624	29.206503
368.779893	19319.049532	29.211520
368.952616	19323.655367	29.216538
369.198155	19325.823769	29.221556
369.272359	19329.073190	29.226573
369.485009	19346.498600	29.231591
369.677515	19353.625343	29.236608
369.718239	19379.748931	29.241626
370.058239	19393.748473	29.246644
370.245802	19424.053601	29.251661
370.440993	19443.602769	29.256679
370.634501	19469.544218	29.261696
370.635717	19515.350527	29.266714
371.088044	19536.522319	29.271732
371.238820	19579.026759	29.276749
371.384022	19626.136287	29.281767
371.908692	19665.762419	29.286784
371.737553	19710.028374	29.291802
372.455092	19747.647578	29.296820
372.740012	19794.366251	29.301837
373.123769	19836.842447	29.306855
373.493955	19876.189660	29.311872
373.688816	19924.738960	29.316890
374.088995	19963.947212	29.321908
374.321779	20014.267271	29.326925
375.285257	20055.135705	29.331943
376.560314	20082.392241	29.336960
376.715022	20122.790814	29.341978
377.222424	20146.665974	29.346996
377.625630	20175.057557	29.352013
377.920143	20208.215487	29.357031
378.739273	20233.305074	29.362048
378.628278	20272.399818	29.367066
379.079904	20294.028370	29.372084
379.298312	20331.564122	29.377101
379.667060	20361.586014	29.382119
380.370033	20392.514102	29.387136
380.513157	20433.501967	29.392154
381.087382	20451.397931	29.397172
381.444634	20495.004578	29.402189
381.892658	20516.979352	29.407207
381.886970	20543.153684	29.412224
382.412140	20574.550928	29.417242
382.961771	20599.944266	29.422260
383.094502	20638.753677	29.427277
383.268762	20678.193095	29.432295
383.864336	20710.343282	29.437312
384.022431	20754.426236	29.442330
384.030107	20789.808904	29.447348
384.405423	20832.790474	29.452365
384.908845	20863.852961	29.457383
385.397072	20907.695245	29.462400
385.802400	20949.232311	29.467418
386.127191	20975.281290	29.472436
386.521749	21010.568154	29.477453
386.631498	21051.705146	29.482471
387.498522	21087.220264	29.487488
387.818771	21113.752752	29.492506
388.381799	21142.090181	29.497524
388.701614	21179.367590	29.502541
389.279348	21191.990698	29.507559
390.266744	21220.928855	29.512576
390.457197	21252.178145	29.517594
391.097287	21261.105467	29.522612
391.544579	21288.072173	29.527629
391.594994	21310.090886	29.532647
392.158590	21322.057379	29.537664
392.809861	21353.117501	29.542682
392.743992	21369.775898	29.547700
393.254060	21394.330420	29.552717
393.494898	21414.563138	29.557735
394.049133	21446.647692	29.562752
394.073707	21474.038782	29.567770
394.339710	21502.413523	29.572788
394.820790	21542.079895	29.577805
394.866268	21568.538761	29.582823
395.744154	21592.945383	29.587840
395.908633	21632.019691	29.592858
395.942522	21662.750955	29.597876
396.679223	21698.877875	29.602893
397.031419	21735.469726	29.607911
397.745487	21762.829849	29.612928
397.767037	21800.249617	29.617946
398.338875	21829.378298	29.622964
398.754315	21867.333096	29.627981
399.009307	21914.163649	29.632999
399.516056	21943.297372	29.638016
399.709843	21983.920745	29.643034
400.171649	22010.548643	29.648052
400.554752	22048.354845	29.653069
400.923046	22084.583565	29.658087
401.474253	22120.654859	29.663104
401.932071	22154.931889	29.668122
401.884842	22191.534820	29.673140
402.443540	22236.114350	29.678157
402.514907	22278.907227	29.683175
403.164520	22310.783096	29.688192
403.217346	22345.965707	29.693210
403.532083	22393.706709	29.698228
403.999732	22445.278939	29.703245
404.631777	22490.332272	29.708263
405.100570	22520.804463	29.713280
405.854758	22566.524633	29.718298
406.415028	22601.377950	29.723316
407.289021	22621.691256	29.728333
407.602559	22656.050788	29.733351
408.251702	22675.219941	29.738368
408.582139	22707.353104	29.743386
409.074107	22735.872527	29.748404
408.882202	22745.427357	29.753421
409.295071	22780.596470	29.758439
409.739280	22796.460764	29.763456
409.572733	22837.242533	29.768474
410.214293	22863.270075	29.773492
410.792792	22890.059127	29.778509
411.124355	22928.021192	29.783527
411.632618	22955.238717	29.788544
411.856666	22994.228652	29.793562
412.639577	23024.818230	29.798580
412.903460	23055.651359	29.803597
412.993092	23097.039583	29.808615
413.724235	23126.174718	29.813632
413.545166	23161.587987	29.818650
414.154063	23197.579123	29.823668
414.556498	23234.006288	29.828685
415.028200	23270.522591	29.833703
415.588319	23299.889194	29.838720
416.035964	23337.472702	29.843738
416.250547	23378.805496	29.848756
416.777699	23411.373080	29.853773
416.818363	23458.429099	29.858791
417.486457	23490.729811	29.863808
417.548668	23540.845050	29.868826
418.244937	23577.538005	29.873844
419.130684	23623.531790	29.878861
418.908498	23657.814808	29.883879
419.910279	23694.051922	29.888896
420.286747	23728.213565	29.893914
420.890360	23760.721396	29.898932
421.667871	23785.947955	29.903949
421.865720	23823.663651	29.908967
422.706110	23847.778703	29.913984
423.179119	23871.142956	29.919002
423.494504	23892.023484	29.924020
424.172393	23911.447745	29.929037
424.442975	23941.928041	29.934055
424.990064	23965.465828	29.939072
425.512254	23986.380425	29.944090
426.043931	24008.135607	29.949108
426.195443	24025.275049	29.954125
426.637912	24059.217859	29.959143
426.945113	24079.538559	29.964160
426.894842	24116.101949	29.969178
427.102556	24149.451157	29.974196
427.528759	24178.419539	29.979213
427.805045	24227.008111	29.984231
428.298253	24259.021655	29.989248
428.739901	24289.413320	29.994266
428.978599	24327.542641	29.999284
429.593824	24362.200860	30.004301
430.034766	24399.273683	30.009319
430.909222	24427.402322	30.014336
431.688964	24461.650875	30.019354
431.829151	24486.990835	30.024372
432.145960	24499.654804	30.029389
432.384137	24526.731845	30.034407
432.760063	24552.952573	30.039424
433.082330	24591.938759	30.044442
433.478439	24625.212440	30.049460
434.158598	24651.188767	30.054477
434.334013	24700.341663	30.059495
434.646792	24721.681029	30.064512
435.210919	24763.493489	30.069530
435.427982	24803.671614	30.074548
436.104320	24831.926343	30.079565
436.442701	24872.449748	30.084583
436.596316	24900.671144	30.089600
436.980646	24937.395221	30.094618
437.114501	24984.187075	30.099636
437.846597	25028.056469	30.104653
437.962071	25070.832953	30.109671
439.034785	25116.833388	30.114688
439.977338	25130.898421	30.119706
440.775435	25160.621727	30.124724
441.684561	25180.827959	30.129741
442.037479	25201.426049	30.134759
442.513848	25225.069158	30.139776
442.800681	25237.060594	30.144794
443.129173	25263.924581	30.149812
443.247864	25281.014113	30.154829
443.684172	25309.149878	30.159847
444.079853	25343.112694	30.164864
444.480963	25378.620352	30.169882
444.611092	25414.253381	30.174900
445.152041	25433.425234	30.179917
445.567537	25475.646582	30.184935
445.756229	25513.512644	30.189952
446.281385	25552.614489	30.194970
446.643627	25588.406836	30.199988
446.886541	25631.882101	30.205005
446.924874	25671.278991	30.210023
447.353306	25708.000300	30.215040
447.941688	25756.530221	30.220058
447.987274	25813.124916	30.225076
448.248366	25856.285323	30.230093
448.562291	25919.651448	30.235111
448.844029	25973.010585	30.240128
449.302071	26037.585896	30.245146
449.936656	26099.241550	30.250164
450.493092	26150.708700	30.255181
451.796975	26194.751212	30.260199
452.479024	26240.402012	30.265216
452.970703	26276.608939	30.270234
453.259854	26318.749883	30.275252
454.093636	26359.046753	30.280269
454.312981	26394.209073	30.285287
454.798219	26430.414269	30.290304
455.583332	26468.230680	30.295322
455.793757	26502.495658	30.300340
456.019297	26533.720126	30.305357
456.462419	26560.714747	30.310375
457.031549	26590.258915	30.315392
457.215509	26624.105935	30.320410
457.462027	26671.116472	30.325428
458.343365	26702.493863	30.330445
458.513664	26748.874103	30.335463
459.095102	26779.161004	30.340480
459.827062	26834.120804	30.345498
459.751535	26870.505032	30.350516
460.575602	26904.110405	30.355533
460.882254	26955.313568	30.360551
461.618072	26980.734922	30.365568
461.974788	27007.817603	30.370586
462.163002	27058.132781	30.375604
462.588356	27098.299444	30.380621
462.865042	27149.744923	30.385639
463.158636	27204.241532	30.390656
463.458404	27253.068003	30.395674
463.963234	27308.481502	30.400692
464.482995	27360.015294	30.405709
464.383054	27416.889359	30.410727
464.694328	27471.352221	30.415744
465.444855	27522.884807	30.420762
465.857781	27599.995390	30.425780
466.213844	27647.942562	30.430797
466.524832	27714.375968	30.435815
466.945459	27785.428594	30.440832
467.540948	27846.207426	30.445850
467.614363	27916.228467	30.450868
468.597706	27979.897498	30.455885
468.879760	28049.334353	30.460903
469.391175	28113.378150	30.465920
469.985251	28169.905412	30.470938
470.368939	28240.881025	30.475956
470.928912	28297.991912	30.480973
471.854488	28362.404198	30.485991
472.362032	28413.908475	30.491008
473.556452	28460.856035	30.496026
474.029604	28503.450278	30.501044
474.977055	28538.589945	30.506061
475.380677	28576.659287	30.511079
475.878396	28620.322330	30.516096
476.776707	28646.800461	30.521114
477.109892	28692.129368	30.526132
477.623761	28728.949660	30.531149
477.755944	28766.964964	30.536167
478.217475	28793.388801	30.541184
478.596629	28838.429403	30.546202
478.899534	28881.429194	30.551220
479.478294	28924.536422	30.556237
479.913450	28976.994985	30.561255
479.976206	29020.093058	30.566272
480.541052	29063.303975	30.571290
480.901934	29109.288639	30.576308
481.335584	29155.065333	30.581325
481.655628	29195.491480	30.586343
482.086952	29254.085212	30.591360
482.624774	29307.338051	30.596378
482.623208	29351.946679	30.601396
483.506788	29398.719682	30.606413
484.623597	29433.153747	30.611431
485.242992	29470.629571	30.616448
486.125318	29503.785065	30.621466
486.482024	29542.180058	30.626484
487.099271	29574.270459	30.631501
488.036419	29595.180650	30.636519
488.323402	29630.135927	30.641536
488.921563	29654.792783	30.646554
488.737135	29695.814517	30.651572
489.393682	29724.919876	30.656589
489.882320	29759.821923	30.661607
489.939641	29798.347655	30.666624
490.460330	29838.352792	30.671642
490.889444	29883.993320	30.676660
491.429706	29925.105969	30.681677
492.152056	29966.338967	30.686695
492.434453	30005.852065	30.691712
493.157374	30043.983454	30.696730
493.608134	30089.197987	30.701748
494.082648	30131.903213	30.706765
494.658162	30175.686146	30.711783
495.223592	30218.252942	30.716800
495.723838	30251.453226	30.721818
496.371697	30299.531159	30.726836
497.282171	30325.533274	30.731853
497.913671	30346.663970	30.736871
498.517187	30377.836810	30.741888
499.249372	30404.216685	30.746906
499.689392	30431.766833	30.751924
499.641478	30464.102200	30.756941
500.103297	30486.659987	30.761959
500.093336	30538.385357	30.766976
500.438366	30564.882298	30.771994
500.981352	30614.411624	30.777012
501.201600	30652.153987	30.782029
501.250571	30700.455535	30.787047
501.444893	30760.978675	30.792064
502.427052	30815.542012	30.797082
502.298344	30869.683699	30.802100
503.503644	30927.074327	30.807117
503.956963	30978.548041	30.812135
503.865414	31040.629447	30.817152
504.475174	31097.781876	30.822170
505.106854	31159.534663	30.827188
505.725182	31220.052976	30.832205
506.379199	31275.844663	30.837223
506.456104	31336.456144	30.842240
507.860558	31369.143849	30.847258
508.438294	31407.874211	30.852276
509.820702	31432.493834	30.857293
510.752745	31450.601788	30.862311
511.288903	31478.487358	30.867328
511.399907	31493.526801	30.872346
512.102025	31523.094338	30.877364
512.987702	31530.885191	30.882381
513.495424	31561.174023	30.887399
513.965985	31579.998617	30.892416
514.492592	31601.063583	30.897434
514.740220	31622.984215	30.902452
515.074860	31648.130792	30.907469
515.434117	31683.882414	30.912487
515.815571	31705.388919	30.917504
515.687365	31728.478551	30.922522
516.239576	31772.600758	30.927540
516.518345	31815.274147	30.932557
517.136510	31845.105903	30.937575
517.041432	31898.749512	30.942592
517.710645	31951.132590	30.947610
517.971917	32003.819242	30.952628
518.663318	32053.191448	30.957645
519.221918	32107.197031	30.962663
518.908009	32166.357243	30.967680
519.727447	32222.975595	30.972698
520.515666	32286.687261	30.977716
520.779951	32346.351742	30.982733
521.273333	32411.862657	30.987751
521.676638	32468.537311	30.992768
522.173888	32533.801859	30.997786
522.883083	32596.938039	31.002804
523.484223	32651.401876	31.007821
524.412353	32706.156990	31.012839
524.794740	32774.190807	31.017856
525.376293	32828.219879	31.022874
525.523974	32892.971270	31.027892
525.862861	32957.058961	31.032909
526.632522	33014.808675	31.037927
527.334777	33083.044479	31.042944
528.046584	33136.651365	31.047962
528.141185	33193.706260	31.052980
528.901803	33260.206462	31.057997
529.738282	33311.113141	31.063015
530.511480	33363.690825	31.068032
531.367312	33406.597343	31.073050
531.802411	33465.933307	31.078068
532.501088	33503.252559	31.083085
533.477279	33539.426066	31.088103
533.948634	33586.940316	31.093120
534.813646	33617.887817	31.098138
535.370982	33651.302412	31.103156
535.722321	33690.628806	31.108173
536.375768	33720.874235	31.113191
536.664483	33759.750736	31.118208
536.842418	33800.473628	31.123226
537.675621	33840.702460	31.128244
537.821596	33885.786315	31.133261
538.387393	33922.100344	31.138279
538.475508	33979.379761	31.143296
538.481005	34017.626798	31.148314
538.789963	34076.954828	31.153332
538.953451	34142.774749	31.158349
539.625404	34195.956085	31.163367
540.085156	34263.161695	31.168384
540.482772	34329.974221	31.173402
541.067827	34398.336088	31.178420
541.489693	34462.541161	31.183437
541.887380	34525.406093	31.188455
542.650837	34601.647423	31.193472
542.976530	34668.801763	31.198490
543.526946	34746.876060	31.203508
543.999799	34819.248139	31.208525
545.214432	34884.603442	31.213543
545.585566	34948.295002	31.218560
546.459611	35006.673927	31.223578
547.086537	35071.240550	31.228596
547.566748	35135.365418	31.233613
548.577483	35186.481099	31.238631
549.161370	35249.928954	31.243648
549.611330	35312.143784	31.248666
550.094881	35367.213573	31.253684
550.205137	35428.619031	31.258701
551.573802	35486.135151	31.263719
552.209214	35549.572069	31.268736
552.481950	35599.404494	31.273754
553.277992	35649.750252	31.278772
553.882302	35706.959308	31.283789
554.459765	35755.010277	31.288807
554.830404	35819.648726	31.293824
555.342790	35868.231943	31.298842
555.948450	35921.966290	31.303860
556.165525	35986.593766	31.308877
556.797575	36041.532839	31.313895
557.331022	36104.689307	31.318912
558.151241	36163.791369	31.323930
558.701559	36212.290096	31.328948
559.092987	36274.451961	31.333965
560.042989	36319.299941	31.338983
560.587447	36382.938423	31.344000
561.047942	36434.852631	31.349018
561.887551	36482.554430	31.354036
561.899398	36545.801796	31.359053
563.005556	36592.381853	31.364071
563.566368	36644.718222	31.369088
564.195355	36696.651654	31.374106
564.623419	36749.961179	31.379124
565.249359	36804.433278	31.384141
565.824435	36855.202171	31.389159
566.073752	36913.151336	31.394176
566.399246	36961.775803	31.399194
567.114834	37006.716144	31.404212
567.707127	37066.668265	31.409229
568.186261	37114.092569	31.414247
569.259791	37157.286341	31.419264
569.158919	37214.229533	31.424282
569.847163	37256.065927	31.429300
570.540769	37320.392356	31.434317
570.812374	37371.028436	31.439335
571.898208	37425.575108	31.444352
572.364897	37475.527787	31.449370
572.991450	37518.379162	31.454388
573.418530	37579.949065	31.459405
574.132497	37617.296268	31.464423
574.675398	37666.219962	31.469440
575.032118	37727.821357	31.474458
575.789331	37780.272533	31.479476
576.102333	37838.718784	31.484493
577.068553	37885.591283	31.489511
577.228908	37948.859082	31.494528
577.453283	38010.329420	31.499546
577.934194	38068.570856	31.504564
578.359209	38132.488425	31.509581
579.280235	38206.025128	31.514599
579.868024	38269.826896	31.519616
580.116809	38338.876727	31.524634
580.784033	38392.437319	31.529652
581.165944	38467.983613	31.534669
581.725009	38536.049763	31.539687
582.160456	38608.380129	31.544704
582.740744	38679.075971	31.549722
584.292217	38738.114727	31.554740
584.487895	38808.943257	31.559757
585.211988	38865.642880	31.564775
586.197605	38929.211457	31.569792
586.524594	38993.426613	31.574810
587.039395	39054.377138	31.579828
587.620444	39121.223113	31.584845
588.588686	39175.075354	31.589863
589.142219	39238.981054	31.594880
589.743137	39304.665691	31.599898
590.613338	39349.361134	31.604916
590.832211	39431.142733	31.609933
591.110146	39486.269605	31.614951
591.851586	39539.975507	31.619968
592.274926	39614.183982	31.624986
592.881253	39667.765025	31.630004
593.204021	39742.486896	31.635021
593.553880	39800.446863	31.640039
594.195023	39882.710586	31.645056
594.711433	39967.310175	31.650074
595.710404	40020.913365	31.655092
596.335470	40093.968437	31.660109
597.564268	40150.165637	31.665127
598.740220	40198.444568	31.670144
599.665512	40240.853299	31.675162
600.230438	40279.541638	31.680180
600.739455	40325.362115	31.685197
601.440229	40361.482706	31.690215
601.735480	40395.933262	31.695232
602.091487	40445.969775	31.700250
602.525172	40492.526557	31.705268
602.648135	40548.857599	31.710285
602.812624	40610.558366	31.715303
603.508846	40674.349852	31.720320
604.081520	40736.666212	31.725338
604.900592	40802.842875	31.730356
605.838682	40863.022768	31.735373
606.413713	40910.721394	31.740391
606.599260	40963.364798	31.745408
606.798325	41036.805970	31.750426
607.740992	41092.714066	31.755444
608.261150	41168.579192	31.760461
608.587950	41231.071936	31.765479
609.394022	41300.469863	31.770496
609.604181	41372.818033	31.775514
610.538194	41439.138286	31.780532
611.475605	41525.646150	31.785549
611.525874	41588.414794	31.790567
612.477958	41660.314917	31.795584
612.863839	41737.746146	31.800602
613.446646	41803.679519	31.805620
613.928162	41881.372807	31.810637
614.408932	41957.235252	31.815655
614.913210	42039.481428	31.820672
615.396918	42132.457284	31.825690
615.946825	42207.374296	31.830708
616.616043	42296.539721	31.835725
617.498204	42371.271009	31.840743
618.714984	42447.606103	31.845760
619.511970	42524.597566	31.850778
620.209104	42588.963783	31.855796
620.990126	42660.417111	31.860813
621.787190	42732.098463	31.865831
622.389746	42797.337289	31.870848
623.125832	42847.113028	31.875866
624.692688	42896.819193	31.880884
625.324576	42952.021964	31.885901
625.879523	42992.261687	31.890919
626.984790	43034.923809	31.895936
627.202908	43086.917135	31.900954
627.652568	43128.135096	31.905972
628.229815	43179.489310	31.910989
628.439172	43233.536987	31.916007
629.117884	43293.731248	31.921024
629.505554	43360.742380	31.926042
629.977839	43414.584491	31.931060
630.140522	43488.770908	31.936077
630.638903	43557.266817	31.941095
631.436390	43613.390458	31.946112
631.814854	43689.871064	31.951130
632.195901	43760.194012	31.956148
632.506474	43829.237788	31.961165
632.925775	43900.363079	31.966183
633.963183	43975.532013	31.971200
634.271677	44064.726560	31.976218
635.114765	44124.816366	31.981236
635.710118	44213.795110	31.986253
636.135864	44283.105010	31.991271
637.196038	44345.618247	31.996288
637.837495	44434.738547	32.001306
638.309294	44509.719143	32.006324
638.915101	44581.433974	32.011341
639.551500	44668.288907	32.016359
640.250596	44744.008322	32.021376
640.631682	44834.908777	32.026394
641.405423	44905.203434	32.031412
641.529533	44988.954967	32.036429
642.579295	45068.660882	32.041447
644.337987	45131.031779	32.046464
644.845804	45219.774443	32.051482
645.673600	45280.271593	32.056500
646.438162	45351.523178	32.061517
647.005427	45419.470844	32.066535
648.524797	45449.517673	32.071552
649.601075	45501.544296	32.076570
650.643964	45538.989972	32.081588
651.154536	45579.334385	32.086605
651.493957	45633.912958	32.091623
652.723516	45674.601785	32.096640
652.871136	45720.345737	32.101658
653.910674	45751.675303	32.106676
655.049704	45787.405976	32.111693
655.816725	45817.317006	32.116711
656.489023	45857.100593	32.121728
656.573249	45900.686256	32.126746
656.947154	45943.843423	32.131764
657.362824	45991.070609	32.136781
657.811280	46045.707475	32.141799
658.620409	46086.721859	32.146816
658.957691	46146.892089	32.151834
659.265688	46198.035329	32.156852
659.892708	46251.524222	32.161869
660.300337	46320.004589	32.166887
660.838639	46383.084501	32.171904
661.126625	46456.376751	32.176922
661.476283	46530.034538	32.181940
661.872943	46614.340245	32.186957
662.321190	46696.575187	32.191975
663.439800	46778.329286	32.196992
663.783994	46864.524214	32.202010
664.362216	46934.888275	32.207028
665.134754	47018.487087	32.212045
665.690010	47107.539900	32.217063
666.523886	47191.782718	32.222080
666.760846	47280.985611	32.227098
667.591097	47348.519244	32.232116
668.712729	47425.992935	32.237133
669.131506	47504.320077	32.242151
670.509615	47558.356670	32.247168
671.179330	47631.575376	32.252186
671.558358	47693.164558	32.257204
672.604548	47761.903885	32.262221
673.021468	47839.613670	32.267239
673.514519	47904.209721	32.272256
674.272963	47986.539167	32.277274
674.866199	48050.092062	32.282292
675.924984	48117.342889	32.287309
676.123207	48200.154547	32.292327
676.883424	48274.124533	32.297344
677.271786	48355.350326	32.302362
677.824774	48437.003078	32.307380
678.461212	48511.055187	32.312397
679.490828	48589.019936	32.317415
680.670509	48658.532377	32.322432
681.856503	48727.153284	32.327450
682.602018	48787.517678	32.332468
683.171473	48860.767701	32.337485
683.570942	48932.486792	32.342503
684.309935	48987.508649	32.347520
685.025278	49054.714186	32.352538
685.520506	49128.338013	32.357556
686.269466	49201.230078	32.362573
686.749236	49276.310072	32.367591
687.212438	49348.910515	32.372608
687.450361	49442.725336	32.377626
688.620580	49522.735511	32.382644
689.019726	49602.745443	32.387661
689.586046	49686.637512	32.392679
690.215647	49769.116642	32.397696
690.631951	49863.313563	32.402714
691.071475	49961.783874	32.407732
692.131709	50051.941943	32.412749
692.744204	50145.601221	32.417767
693.783970	50220.999566	32.422784
694.401228	50317.154278	32.427802
695.050251	50395.658985	32.432820
696.515423	50466.316707	32.437837
697.386176	50556.926535	32.442855
698.049806	50627.993812	32.447872
698.688887	50706.267718	32.452890
699.403504	50783.252820	32.457908
700.194468	50870.876859	32.462925
700.843550	50943.072332	32.467943
701.940453	51009.530618	32.472960
702.468978	51079.624471	32.477978
703.029277	51157.477750	32.482996
703.727698	51230.322886	32.488013
703.899406	51308.622405	32.493031
704.771606	51387.478254	32.498048
705.371218	51478.600007	32.503066
705.868530	51563.604961	32.508084
706.503308	51634.813512	32.513101
707.084980	51705.247986	32.518119
708.333731	51769.547352	32.523136
708.748476	51857.764648	32.528154
709.360144	51935.214175	32.533172
709.791086	52015.095848	32.538189
710.505014	52099.699562	32.543207
711.597324	52173.377899	32.548224
712.223187	52256.045059	32.553242
712.545554	52345.335501	32.558260
713.295073	52429.688126	32.563277
713.850835	52521.213951	32.568295
715.127404	52596.700926	32.573312
715.648868	52679.969031	32.578330
716.012997	52772.002720	32.583348
716.993221	52861.252305	32.588365
717.657747	52956.836874	32.593383
718.494679	53039.117328	32.598400
719.223572	53117.069527	32.603418
720.137022	53199.084800	32.608436
720.865933	53278.705716	32.613453
721.633044	53372.158016	32.618471
722.624298	53447.475972	32.623488
723.504324	53539.336395	32.628506
723.687076	53626.691454	32.633524
724.580196	53700.245329	32.638541
725.174277	53790.803709	32.643559
725.890747	53883.616271	32.648576
726.656288	53967.454575	32.653594
727.619659	54051.379401	32.658612
728.592709	54135.246055	32.663629
729.256388	54218.072904	32.668647
730.031041	54299.920624	32.673664
730.863628	54374.207713	32.678682
731.251398	54458.795239	32.683700
732.230089	54535.111541	32.688717
732.346842	54628.074541	32.693735
733.158053	54720.249201	32.698752
733.518738	54815.484032	32.703770
734.519165	54895.627308	32.708788
736.141136	54968.214273	32.713805
736.877915	55046.134778	32.718823
738.252976	55120.104237	32.723840
739.683618	55189.691618	32.728858
740.563192	55244.201382	32.733876
741.526266	55291.644815	32.738893
742.285539	55336.564008	32.743911
743.064465	55388.772273	32.748928
743.984260	55455.124198	32.753946
744.216366	55512.987358	32.758964
745.043874	55562.432574	32.763981
745.162871	55629.794307	32.768999
745.970719	55696.602238	32.774016
746.546886	55746.242625	32.779034
746.899762	55807.555242	32.784052
747.810232	55856.784757	32.789069
748.485120	55927.565817	32.794087
748.467172	55990.244299	32.799104
749.514674	56064.260727	32.804122
750.043712	56145.058507	32.809140
750.604720	56213.117451	32.814157
751.503561	56288.582047	32.819175
752.083148	56367.166566	32.824192
752.782437	56449.699545	32.829210
753.055786	56537.108678	32.834228
753.621085	56613.042396	32.839245
754.563688	56705.178408	32.844263
754.887439	56802.786212	32.849280
755.837965	56891.913579	32.854298
756.267276	56990.755502	32.859316
757.341706	57080.127904	32.864333
757.862545	57176.920112	32.869351
758.631523	57276.406742	32.874368
759.389736	57374.239916	32.879386
760.181725	57478.665690	32.884404
761.309983	57566.425784	32.889421
762.228048	57658.184839	32.894439
762.761389	57752.746738	32.899456
764.012999	57841.049369	32.904474
764.546171	57941.413894	32.909492
765.401130	58025.563524	32.914509
766.114671	58128.072161	32.919527
766.619890	58220.498563	32.924544
767.296574	58320.695020	32.929562
767.521234	58429.691183	32.934580
768.445106	58530.598429	32.939597
769.010425	58638.601974	32.944615
770.081815	58743.864908	32.949632
771.255466	58849.926185	32.954650
772.068345	58959.620781	32.959668
772.821150	59054.998066	32.964685
773.688479	59151.765620	32.969703
774.841008	59233.707716	32.974720
776.167679	59323.078398	32.979738
776.887649	59414.158786	32.984756
777.712702	59499.596365	32.989773
778.340912	59594.523478	32.994791
779.065044	59684.447707	32.999808
779.480201	59779.968380	33.004826
779.785853	59874.117726	33.009844
780.740147	59965.710324	33.014861
781.497376	60071.539566	33.019879
782.039896	60177.254436	33.024896
783.255126	60268.595109	33.029914
784.069281	60370.996646	33.034932
784.893646	60455.528144	33.039949
785.601960	60560.401209	33.044967
786.660376	60657.250603	33.049984
787.446417	60742.820142	33.055002
787.949914	60833.311829	33.060020
788.650323	60925.710704	33.065037
789.697447	61003.272267	33.070055
790.548172	61085.943489	33.075072
791.492150	61162.132709	33.080090
791.908267	61263.715609	33.085108
793.024518	61343.131310	33.090125
793.445425	61431.686572	33.095143
793.913610	61525.240416	33.100160
795.005916	61618.491826	33.105178
795.400500	61717.248785	33.110196
795.948692	61812.199839	33.115213
796.833669	61917.732234	33.120231
797.613648	62020.830511	33.125248
798.762062	62119.302236	33.130266
799.156788	62221.310706	33.135284
800.245578	62318.339690	33.140301
800.739968	62428.233771	33.145319
801.690794	62534.263736	33.150336
802.483263	62638.456545	33.155354
803.024144	62742.680327	33.160372
804.049904	62852.675281	33.165389
804.934484	62954.306334	33.170407
805.600629	63072.417669	33.175424
806.502610	63173.939347	33.180442
807.535358	63292.159817	33.185460
808.041037	63397.827916	33.190477
808.886429	63504.140069	33.195495
809.857342	63608.300844	33.200512
810.799162	63707.276963	33.205530
811.756890	63824.931700	33.210548
812.808661	63915.267056	33.215565
814.054604	64015.406333	33.220583
814.657607	64118.501057	33.225600
815.646904	64206.016170	33.230618
816.822760	64298.019874	33.235636
817.385261	64391.956085	33.240653
818.324564	64489.438032	33.245671
818.799048	64582.637855	33.250688
819.786810	64677.975537	33.255706
820.250778	64783.746281	33.260724
820.779138	64875.098449	33.265741
822.197271	64977.273836	33.270759
822.842796	65082.363805	33.275776
823.817586	65181.745858	33.280794
824.754036	65262.983846	33.285812
825.444853	65366.961089	33.290829
826.586536	65457.964169	33.295847
827.025546	65556.396582	33.300864
828.280449	65647.463279	33.305882
828.809708	65753.708205	33.310900
829.827894	65841.168277	33.315917
830.596361	65946.715675	33.320935
830.793504	66048.296115	33.325952
831.702787	66146.600148	33.330970
832.442020	66238.668154	33.335988
833.739164	66332.095187	33.341005
834.632381	66428.683552	33.346023
834.568828	66516.736338	33.351040
836.060599	66606.008914	33.356058
836.603414	66694.888007	33.361076
837.568141	66798.250009	33.366093
838.332840	66891.024626	33.371111
838.426937	67004.280039	33.376128
840.059207	67097.924925	33.381146
840.382955	67199.855909	33.386164
841.022906	67303.155858	33.391181
841.617051	67419.837002	33.396199
842.373826	67534.922852	33.401216
843.941489	67618.641507	33.406234
845.546877	67720.273268	33.411252
847.029081	67811.835136	33.416269
848.730326	67889.879239	33.421287
849.453736	67968.078460	33.426304
850.286113	68026.145698	33.431322
850.768444	68106.808442	33.436340
851.965644	68194.241220	33.441357
852.711508	68279.298289	33.446375
853.052943	68358.247255	33.451392
853.716114	68440.252404	33.456410
854.363925	68548.103382	33.461428
854.892135	68639.623527	33.466445
855.629485	68738.164990	33.471463
855.944498	68841.907421	33.476480
856.842408	68938.481055	33.481498
857.452070	69051.817084	33.486516
858.208361	69167.835001	33.491533
859.181700	69285.163257	33.496551
860.015252	69402.857559	33.501568
860.841888	69509.525541	33.506586
861.194370	69627.075815	33.511604
862.058867	69756.180688	33.516621
862.929728	69876.533399	33.521639
863.415899	70007.955769	33.526656
864.228996	70137.090692	33.531674
865.408704	70257.525424	33.536692
866.592277	70382.070591	33.541709
867.604640	70508.909707	33.546727
868.628786	70623.605842	33.551744
869.483859	70754.210700	33.556762
870.177116	70871.178158	33.561780
870.787056	70997.665354	33.566797
871.795872	71119.885868	33.571815
872.516371	71254.279527	33.576832
873.409178	71375.673933	33.581850
874.209491	71508.366977	33.586868
874.743269	71632.100962	33.591885
875.868263	71761.217415	33.596903
876.865433	71890.698029	33.601920
878.406568	72003.643313	33.606938
879.393855	72112.718742	33.611956
880.560521	72218.165486	33.616973
881.557878	72318.266086	33.621991
882.356678	72419.918987	33.627008
883.705523	72512.143414	33.632026
884.393589	72612.108598	33.637044
885.525798	72714.660747	33.642061
887.196419	72793.720757	33.647079
888.471228	72874.056812	33.652096
889.544616	72951.044064	33.657114
889.846597	73036.271710	33.662132
890.682634	73105.976384	33.667149
891.821286	73195.943888	33.672167
892.372250	73294.379821	33.677184
893.131458	73377.822848	33.682202
893.876052	73474.499809	33.687220
894.419084	73575.651623	33.692237
894.828059	73669.401680	33.697255
895.388719	73777.091121	33.702272
896.219522	73887.207795	33.707290
897.390966	73993.712156	33.712308
898.487014	74101.735246	33.717325
899.623603	74199.170473	33.722343
900.829792	74306.062529	33.727360
901.611618	74413.590695	33.732378
902.636427	74512.526471	33.737396
902.861592	74621.365366	33.742413
903.483578	74729.485359	33.747431
904.581295	74851.584920	33.752448
905.509722	74963.132331	33.757466
905.880524	75087.388021	33.762484
906.698203	75214.667182	33.767501
907.603081	75323.291901	33.772519
908.242889	75464.821905	33.777536
909.075761	75586.205507	33.782554
909.996450	75707.511477	33.787572
911.213547	75839.994749	33.792589
912.041465	75962.323715	33.797607
912.921030	76096.422346	33.802624
913.812675	76220.335804	33.807642
914.926669	76356.350396	33.812660
915.232715	76487.779046	33.817677
916.789810	76618.222499	33.822695
917.621302	76758.469081	33.827712
918.743685	76873.142945	33.832730
919.802137	76997.645715	33.837748
920.530657	77134.053644	33.842765
921.323618	77261.083000	33.847783
921.999620	77394.281719	33.852800
923.054818	77525.195937	33.857818
923.814896	77665.529986	33.862836
925.012040	77794.201096	33.867853
926.096651	77928.281867	33.872871
927.101625	78056.152364	33.877888
928.099814	78175.200035	33.882906
929.722769	78281.698120	33.887924
930.340005	78395.820990	33.892941
931.448345	78510.549870	33.897959
932.182698	78623.028032	33.902976
933.228385	78724.528240	33.907994
934.604309	78823.922680	33.913012
935.686436	78935.286368	33.918029
936.780844	79022.672217	33.923047
937.699420	79126.150784	33.928064
938.121437	79221.047899	33.933082
938.857424	79330.536969	33.938100
939.886815	79446.916280	33.943117
940.733327	79558.658664	33.948135
941.425401	79684.105664	33.953152
942.314579	79795.386402	33.958170
942.829137	79910.394844	33.963188
943.281897	80043.546118	33.968205
944.949847	80175.028637	33.973223
945.367542	80308.149495	33.978240
945.991557	80444.146022	33.983258
947.402361	80567.481906	33.988276
948.533749	80700.160160	33.993293
949.423946	80831.887195	33.998311
950.113613	80973.411470	34.003328
950.828074	81106.530420	34.008346
952.246324	81245.476812	34.013364
952.544696	81386.899814	34.018381
953.402020	81526.222338	34.023399
954.292324	81683.211153	34.028416
954.864334	81836.857961	34.033434
955.907667	81983.041455	34.038452
956.966010	82142.636647	34.043469
957.927844	82299.794554	34.048487
958.433019	82467.098205	34.053504
958.951013	82627.915502	34.058522
959.960772	82796.577714	34.063540
960.327826	82970.514268	34.068557
961.543394	83150.419009	34.073575
961.789236	83328.656264	34.078592
962.820552	83517.460041	34.083610
964.166157	83690.740849	34.088628
964.995197	83883.625479	34.093645
966.414289	84058.048034	34.098663
967.363907	84246.422428	34.103680
968.218721	84436.592645	34.108698
969.585799	84607.775774	34.113716
969.756279	84797.003041	34.118733
970.947008	84983.817063	34.123751
972.388071	85174.278848	34.128768
972.524670	85369.945631	34.133786
974.349918	85536.380715	34.138804
975.815593	85717.395014	34.143821
977.362237	85884.196661	34.148839
979.022203	86027.211727	34.153856
980.114029	86180.108251	34.158874
981.737552	86314.841434	34.163892
982.211837	86471.807027	34.168909
983.249172	86609.616527	34.173927
983.957979	86747.774187	34.178944
984.667568	86894.956710	34.183962
985.407422	87043.122186	34.188980
985.826741	87200.083004	34.193997
986.874696	87353.412256	34.199015
987.800576	87500.593119	34.204032
988.722040	87669.336951	34.209050
989.819555	87820.471039	34.214068
991.282682	87980.346577	34.219085
992.733714	88135.991381	34.224103
994.104681	88286.594277	34.229120
994.913954	88439.237225	34.234138
995.689920	88577.115483	34.239156
996.160450	88736.071149	34.244173
996.953320	88900.326880	34.249191
997.902027	89067.208853	34.254208
998.502962	89240.733637	34.259226
999.356005	89408.241926	34.264244
1000.189127	89594.210260	34.269261
1000.897401	89769.619167	34.274279
1001.749182	89959.549116	34.279296
1002.673544	90137.132544	34.284314
1004.121113	90324.064557	34.289332
1004.970716	90518.005646	34.294349
1006.215082	90704.367765	34.299367
1007.609084	90885.578891	34.304384
1008.458697	91074.435586	34.309402
1010.217293	91229.053896	34.314420
1011.166071	91401.382568	34.319437
1012.667835	91568.111050	34.324455
1013.517276	91743.212493	34.329472
1014.069976	91916.365831	34.334490
1015.469878	92080.671998	34.339508
1016.325940	92266.055443	34.344525
1017.731446	92419.450459	34.349543
1019.274530	92587.470060	34.354560
1020.283277	92754.721444	34.359578
1021.699669	92906.180690	34.364596
1022.917234	93053.047731	34.369613
1024.341591	93205.089801	34.374631
1025.427242	93342.372252	34.379648
1027.075269	93463.398573	34.384666
1028.525862	93589.447389	34.389684
1029.628956	93729.514231	34.394701
1030.408050	93855.217283	34.399719
1031.396506	93992.614930	34.404736
1032.173262	94115.122959	34.409754
1032.958785	94249.708183	34.414772
1034.240844	94383.487459	34.419789
1035.054375	94514.828219	34.424807
1036.674396	94641.834558	34.429824
1037.595050	94760.155756	34.434842
1038.546608	94871.762001	34.439860
1039.225951	95001.330465	34.444877
1040.095924	95111.964205	34.449895
1041.187897	95237.506700	34.454912
1042.102502	95374.557430	34.459930
1042.373528	95498.393290	34.464948
1043.788888	95640.107642	34.469965
1044.084670	95781.849903	34.474983
1045.051095	95918.768116	34.480000
1045.397360	96075.722298	34.485018
1046.457510	96221.571387	34.490036
1046.913746	96388.511247	34.495053
1047.690890	96566.488858	34.500071
1048.702612	96734.386802	34.505088
1049.186035	96922.268033	34.510106
1050.285888	97110.070430	34.515124
1051.067286	97299.593798	34.520141
1051.759951	97499.200148	34.525159
1052.726836	97696.057728	34.530176
1053.800171	97890.967599	34.535194
1055.158771	98085.855440	34.540212
1057.296394	98260.566653	34.545229
1058.280642	98444.834197	34.550247
1059.611439	98633.684597	34.555264
1060.767113	98821.097496	34.560282
1062.204883	98994.059466	34.565300
1062.911254	99179.855094	34.570317
1064.043709	99364.268483	34.575335
1065.225201	99543.558897	34.580352
1066.051764	99730.363630	34.585370
1067.225668	99915.388031	34.590388
1068.422697	100102.321970	34.595405
1068.653445	100291.410879	34.600423
1069.880437	100480.989090	34.605440
1070.643676	100691.562154	34.610458
1071.585227	100890.303749	34.615476
1072.582178	101095.502285	34.620493
1073.216015	101307.444859	34.625511
1074.510402	101513.608877	34.630528
1075.384831	101723.341744	34.635546
1076.388417	101930.584642	34.640564
1077.425102	102162.924330	34.645581
1078.422122	102381.303920	34.650599
1080.075052	102591.087737	34.655616
1080.936611	102812.014356	34.660634
1082.340340	103012.333009	34.665652
1083.073547	103241.707301	34.670669
1084.254093	103455.302367	34.675687
1085.626975	103668.524267	34.680704
1086.756093	103877.597437	34.685722
1088.390640	104080.164400	34.690740
1089.861962	104288.586946	34.695757
1091.051826	104480.226859	34.700775
1092.274308	104671.457268	34.705792
1093.446468	104860.569831	34.710810
1094.697371	105040.360910	34.715828
1096.272991	105211.193508	34.720845
1097.482902	105385.319627	34.725863
1098.743236	105548.659469	34.730880
1099.968779	105725.900964	34.735898
1101.133877	105890.513138	34.740916
1102.732811	106052.126138	34.745933
1103.470871	106207.225022	34.750951
1104.084419	106369.819290	34.755968
1104.525997	106549.062398	34.760986
1105.480295	106732.487540	34.766004
1106.672167	106906.081930	34.771021
1107.758701	107079.264802	34.776039
1109.290703	107257.337899	34.781056
1110.925945	107436.103836	34.786074
1111.433012	107608.895296	34.791092
1112.789220	107792.968152	34.796109
1113.735484	107974.819689	34.801127
1114.707329	108149.840424	34.806144
1115.510304	108341.586709	34.811162
1116.698141	108528.530837	34.816180
1117.995102	108709.301161	34.821197
1119.096535	108897.504017	34.826215
1120.736367	109077.394673	34.831232
1121.807198	109257.561279	34.836250
1123.288604	109437.291403	34.841268
1124.557723	109609.838343	34.846285
1125.949842	109781.047836	34.851303
1127.472063	109952.907524	34.856320
1128.493144	110116.100403	34.861338
1129.512489	110284.868554	34.866356
1130.954796	110448.409326	34.871373
1132.481276	110608.845574	34.876391
1134.061505	110768.374089	34.881408
1134.975839	110931.830749	34.886426
1136.296216	111077.799562	34.891444
1137.371632	111236.353034	34.896461
1138.599772	111389.066321	34.901479
1139.585017	111533.777356	34.906496
1140.315119	111703.148396	34.911514
1141.186059	111865.832492	34.916532
1142.350992	112028.441860	34.921549
1142.821448	112197.176215	34.926567
1143.746744	112367.949460	34.931584
1144.916186	112553.188215	34.936602
1145.471181	112734.732593	34.941620
1147.071730	112913.653938	34.946637
1147.544641	113097.913289	34.951655
1148.770546	113276.254932	34.956672
1149.566407	113487.675763	34.961690
1150.798245	113680.132937	34.966708
1152.231160	113868.299929	34.971725
1153.432135	114061.271766	34.976743
1154.901737	114248.535433	34.981760
1155.734939	114444.284212	34.986778
1156.990545	114622.920644	34.991796
1158.143545	114791.895698	34.996813
1159.265524	114973.344652	35.001831
1160.361078	115147.716530	35.006848
1161.439289	115332.254157	35.011866
1162.343491	115520.370519	35.016884
1163.241594	115707.602211	35.021901
1164.013902	115906.298322	35.026919
1165.555714	116107.879716	35.031936
1166.461823	116308.747744	35.036954
1167.272789	116511.027266	35.041972
1168.321141	116720.857539	35.046989
1168.928026	116939.178573	35.052007
1170.066389	117153.874971	35.057024
1170.860595	117379.731995	35.062042
1171.954724	117611.609055	35.067060
1172.892132	117844.097682	35.072077
1174.498611	118073.026916	35.077095
1175.582458	118298.207871	35.082112
1176.831874	118526.694911	35.087130
1178.365516	118764.182854	35.092148
1179.584873	118993.730444	35.097165
1180.559904	119222.497960	35.102183
1182.348998	119451.508049	35.107200
1183.751916	119677.139144	35.112218
1184.983593	119902.205669	35.117236
1186.413363	120126.682396	35.122253
1187.674971	120357.348517	35.127271
1188.912484	120575.753332	35.132288
1190.211127	120793.693059	35.137306
1191.359610	121009.961911	35.142324
1192.785574	121232.014413	35.147341
1193.482535	121456.360468	35.152359
1194.680156	121681.028029	35.157376
1195.854697	121899.174469	35.162394
1197.119031	122136.976233	35.167412
1198.207137	122354.494422	35.172429
1199.465796	122598.130598	35.177447
1201.317917	122818.702404	35.182464
1202.243833	123036.924970	35.187482
1203.195656	123277.121168	35.192500
1204.645022	123499.566562	35.197517
1205.940853	123724.954899	35.202535
1207.441093	123948.611570	35.207552
1208.426175	124180.038667	35.212570
1209.385954	124399.595980	35.217588
1210.828385	124627.412015	35.222605
1212.002838	124859.686354	35.227623
1213.448982	125077.048596	35.232640
1214.962227	125309.534494	35.237658
1216.359263	125523.752284	35.242676
1217.689524	125747.451137	35.247693
1218.431007	125977.323719	35.252711
1219.837239	126191.113597	35.257728
1221.256567	126416.094877	35.262746
1222.571210	126614.249509	35.267764
1223.999730	126799.799303	35.272781
1225.317508	126993.963082	35.277799
1226.539313	127175.266206	35.282816
1227.996149	127370.726766	35.287834
1229.192417	127562.354405	35.292852
1230.598847	127752.945855	35.297869
1231.178576	127950.512231	35.302887
1232.442875	128149.749951	35.307904
1233.422245	128349.101084	35.312922
1234.432385	128556.370725	35.317940
1235.620125	128756.854950	35.322957
1236.165383	128986.187370	35.327975
1237.324255	129201.447124	35.332992
1238.518410	129439.557806	35.338010
1239.561062	129662.294281	35.343028
1241.040259	129876.286810	35.348045
1242.367323	130111.565550	35.353063
1243.788864	130337.081428	35.358080
1245.113235	130575.190940	35.363098
1246.058585	130802.743832	35.368116
1247.237895	131036.482692	35.373133
1248.093100	131275.780588	35.378151
1249.474538	131506.864082	35.383168
1250.885544	131754.944410	35.388186
1251.895301	132005.529379	35.393204
1253.435880	132247.366681	35.398221
1254.457133	132488.064951	35.403239
1256.082010	132726.823398	35.408256
1257.385402	132970.697048	35.413274
1258.949782	133211.662636	35.418292
1260.053197	133450.972020	35.423309
1260.839934	133706.438470	35.428327
1261.836626	133954.416204	35.433344
1263.069997	134217.733987	35.438362
1263.991713	134470.216513	35.443380
1265.507257	134726.478905	35.448397
1266.654240	134985.037782	35.453415
1268.019144	135246.731017	35.458432
1269.462714	135501.857927	35.463450
1270.614390	135764.238321	35.468468
1272.105520	136021.262864	35.473485
1273.830790	136275.396508	35.478503
1275.485278	136519.388211	35.483520
1277.536174	136756.682595	35.488538
1278.155384	137005.863311	35.493556
1279.775691	137249.485746	35.498573
1280.621927	137499.899159	35.503591
1281.907911	137735.556191	35.508608
1283.465249	137990.847231	35.513626
1284.010456	138250.104678	35.518644
1285.715557	138495.230376	35.523661
1286.463973	138760.555896	35.528679
1287.336277	139012.649647	35.533696
1289.055391	139270.686746	35.538714
1290.224496	139524.267718	35.543732
1291.106772	139769.517951	35.548749
1292.427563	140021.757837	35.553767
1293.683393	140265.273806	35.558784
1295.109544	140514.925084	35.563802
1296.310590	140767.875611	35.568820
1297.964304	141005.977383	35.573837
1298.728283	141275.719636	35.578855
1299.988921	141530.808519	35.583872
1301.158835	141786.561509	35.588890
1302.480434	142055.707028	35.593908
1304.170861	142307.291353	35.598925
1305.331181	142577.229307	35.603943
1306.508368	142844.566727	35.608960
1307.945519	143112.495726	35.613978
1309.017004	143377.420372	35.618996
1310.446453	143643.997731	35.624013
1311.567162	143923.641442	35.629031
1312.673220	144204.266336	35.634048
1313.927058	144478.197380	35.639066
1315.384351	144764.080250	35.644084
1316.614018	145041.063385	35.649101
1317.693946	145319.773684	35.654119
1318.667195	145622.879928	35.659136
1320.319014	145920.888306	35.664154
1321.425712	146217.889026	35.669172
1322.519608	146505.762788	35.674189
1324.496004	146801.249612	35.679207
1325.946535	147086.251270	35.684224
1327.892844	147368.202435	35.689242
1329.446507	147658.035732	35.694260
1330.702617	147931.155038	35.699277
1332.319045	148209.300659	35.704295
1334.796639	148464.432824	35.709312
1336.664827	148711.883396	35.714330
1338.224868	148960.352289	35.719348
1340.627761	149190.591718	35.724365
1342.708104	149414.812275	35.729383
1344.110329	149628.838334	35.734400
1346.430684	149828.616718	35.739418
1347.855089	150041.474394	35.744436
1349.883002	150227.073601	35.749453
1351.497475	150415.801326	35.754471
1353.009377	150600.184215	35.759488
1354.359415	150775.907062	35.764506
1355.325813	150960.499212	35.769524
1356.587518	151138.293677	35.774541
1357.241246	151327.329856	35.779559
1358.022635	151524.260165	35.784576
1359.361538	151729.302891	35.789594
1359.827476	151938.136578	35.794612
1360.823339	152156.229226	35.799629
1361.857189	152378.274209	35.804647
1362.720511	152601.224891	35.809664
1364.020853	152832.727714	35.814682
1364.783482	153065.313362	35.819700
1365.905572	153286.561934	35.824717
1366.747624	153528.257212	35.829735
1367.552248	153767.524835	35.834752
1368.859290	154010.653006	35.839770
1369.772803	154272.256352	35.844788
1370.929556	154527.933783	35.849805
1371.900118	154800.909605	35.854823
1372.800344	155087.422106	35.859840
1374.126775	155368.472318	35.864858
1374.729682	155667.636674	35.869876
1375.570208	155960.242074	35.874893
1376.720343	156277.927373	35.879911
1377.561617	156599.879780	35.884928
1378.765835	156925.679935	35.889946
1380.183216	157266.707720	35.894964
1381.488079	157589.768408	35.899981
1383.193767	157921.732329	35.904999
1384.535119	158261.715731	35.910016
1386.275847	158589.568595	35.915034
1387.910901	158922.757874	35.920052
1389.806225	159258.835931	35.925069
1391.618909	159580.201318	35.930087
1393.007436	159906.513582	35.935104
1394.683108	160223.872877	35.940122
1396.028188	160545.871225	35.945140
1397.760212	160875.545054	35.950157
1399.590084	161192.682225	35.955175
1401.099018	161500.792438	35.960192
1403.432588	161812.265508	35.965210
1404.653380	162123.918608	35.970228
1406.227472	162425.655098	35.975245
1407.701767	162739.565747	35.980263
1408.608878	163052.548021	35.985280
1410.077289	163360.018686	35.990298
1411.376437	163673.445846	35.995316
1412.636962	163982.402919	36.000333
1414.158041	164295.225571	36.005351
1415.581213	164618.217926	36.010368
1417.009580	164926.252014	36.015386
1418.500820	165245.583009	36.020404
1420.005719	165558.518865	36.025421
1421.678356	165868.446346	36.030439
1423.006810	166192.621013	36.035456
1424.656168	166497.455902	36.040474
1426.335787	166802.414562	36.045492
1428.182329	167103.641488	36.050509
1430.707022	167381.647335	36.055527
1432.559944	167665.695737	36.060544
1434.215879	167940.859011	36.065562
1435.715595	168217.053136	36.070580
1437.061459	168488.935444	36.075597
1439.118302	168758.756170	36.080615
1440.498181	169017.070619	36.085632
1442.405997	169261.248649	36.090650
1444.276008	169487.617995	36.095668
1445.934270	169707.870115	36.100685
1447.457016	169930.557543	36.105703
1448.233130	170165.822648	36.110720
1449.485612	170387.200670	36.115738
1450.227268	170630.582907	36.120756
1451.551490	170870.300766	36.125773
1452.709464	171118.296921	36.130791
1453.633857	171375.978950	36.135808
1454.769321	171632.065336	36.140826
1455.988312	171895.169283	36.145844
1457.449610	172164.971849	36.150861
1458.885549	172434.627980	36.155879
1460.203927	172706.222020	36.160896
1461.196683	172994.066636	36.165914
1462.521712	173280.472796	36.170932
1463.493406	173564.682134	36.175949
1465.005498	173865.425747	36.180967
1465.584408	174173.310954	36.185984
1467.281431	174488.062971	36.191002
1468.541983	174795.302369	36.196020
1470.117392	175125.143652	36.201037
1471.199471	175438.852023	36.206055
1472.236493	175777.572144	36.211072
1473.951363	176106.215714	36.216090
1474.871792	176449.250022	36.221108
1476.818825	176784.369043	36.226125
1479.207226	177107.827171	36.231143
1480.384037	177447.549851	36.236160
1482.012492	177775.241705	36.241178
1483.640595	178099.001184	36.246196
1485.593327	178431.160048	36.251213
1487.349872	178769.967218	36.256231
1488.697242	179095.481688	36.261248
1490.530314	179405.227366	36.266266
1492.558181	179720.043866	36.271284
1494.075512	180032.715737	36.276301
1495.848873	180337.958582	36.281319
1497.034667	180663.319960	36.286336
1498.847035	180968.064717	36.291354
1500.921153	181250.871420	36.296372
1502.648179	181551.293164	36.301389
1504.710903	181842.012534	36.306407
1505.986774	182137.488346	36.311424
1507.489024	182429.944157	36.316442
1509.122075	182724.676593	36.321460
1510.339663	183015.635678	36.326477
1512.558563	183290.837670	36.331495
1513.835911	183591.576025	36.336512
1515.114486	183879.673214	36.341530
1516.565440	184171.410786	36.346548
1517.666318	184464.542596	36.351565
1519.408383	184750.051625	36.356583
1520.320458	185045.998646	36.361600
1522.683163	185329.639974	36.366618
1524.236156	185609.993965	36.371636
1525.592651	185887.171423	36.376653
1527.022509	186183.746579	36.381671
1527.945334	186513.858537	36.386688
1529.156106	186799.290978	36.391706
1530.591995	187083.962731	36.396724
1531.884062	187371.313553	36.401741
1533.071024	187668.166323	36.406759
1534.641738	187974.678714	36.411776
1535.759205	188279.772320	36.416794
1537.508504	188587.514050	36.421812
1538.362114	188907.038752	36.426829
1539.922989	189223.790969	36.431847
1541.062069	189548.195692	36.436864
1542.742724	189884.188556	36.441882
1544.114440	190206.284636	36.446900
1545.312814	190558.638372	36.451917
1546.948283	190893.641613	36.456935
1548.523178	191246.569584	36.461952
1549.627714	191583.762066	36.466970
1551.487530	191931.490983	36.471988
1553.184088	192290.370707	36.477005
1554.607153	192631.843343	36.482023
1556.257075	192988.360991	36.487040
1558.097466	193341.344116	36.492058
1559.841154	193692.098635	36.497076
1561.703155	194031.434259	36.502093
1563.939296	194370.567983	36.507111
1565.843960	194717.656866	36.512128
1567.212136	195054.327352	36.517146
1568.803192	195392.421426	36.522164
1570.186527	195733.739415	36.527181
1571.962768	196080.743149	36.532199
1573.083793	196415.736160	36.537216
1574.427198	196761.141596	36.542234
1576.385908	197110.607811	36.547252
1578.245333	197457.591663	36.552269
1579.543173	197810.107335	36.557287
1580.851527	198169.085406	36.562304
1582.347035	198517.609610	36.567322
1584.138219	198877.156214	36.572340
1585.046260	199254.084872	36.577357
1586.754051	199613.484435	36.582375
1588.854198	199954.560970	36.587392
1590.339989	200319.791711	36.592410
1592.692952	200666.148255	36.597428
1594.290012	201024.202558	36.602445
1596.062914	201366.839954	36.607463
1597.994183	201698.811848	36.612480
1600.225877	202031.000460	36.617498
1602.443791	202350.165783	36.622516
1604.207754	202681.294589	36.627533
1606.019740	202993.561416	36.632551
1607.977614	203304.649123	36.637568
1609.583026	203610.909979	36.642586
1611.013097	203902.346258	36.647604
1612.351890	204198.433775	36.652621
1614.082610	204485.110103	36.657639
1615.263035	204784.617142	36.662656
1616.734203	205071.047986	36.667674
1618.811785	205365.172376	36.672692
1619.892336	205666.744148	36.677709
1621.371941	205963.042764	36.682727
1622.872408	206268.405021	36.687744
1623.763830	206580.234186	36.692762
1625.150092	206887.611854	36.697780
1626.539166	207211.636998	36.702797
1628.073110	207545.035032	36.707815
1629.297103	207874.970123	36.712832
1630.570525	208219.957822	36.717850
1631.832540	208566.802796	36.722868
1633.111409	208937.569433	36.727885
1634.979586	209289.773803	36.732903
1635.788211	209655.798727	36.737920
1637.330269	210040.010528	36.742938
1638.794862	210425.634083	36.747956
1639.984659	210825.274502	36.752973
1641.401819	211209.208010	36.757991
1643.355362	211608.238719	36.763008
1645.252336	212003.242748	36.768026
1647.227232	212392.343030	36.773044
1648.873856	212801.742696	36.778061
1650.960333	213182.496930	36.783079
1652.713135	213582.535648	36.788096
1654.288247	213980.676248	36.793114
1656.185500	214374.953748	36.798132
1657.587257	214774.168606	36.803149
1659.480264	215166.113464	36.808167
1661.393949	215558.386523	36.813184
1663.604755	215939.765339	36.818202
1665.723475	216323.777374	36.823220
1666.938011	216725.825923	36.828237
1668.495261	217117.835876	36.833255
1670.022634	217510.487394	36.838272
1671.680237	217905.556370	36.843290
1673.837735	218288.273773	36.848308
1675.397006	218685.648367	36.853325
1676.871535	219074.174751	36.858343
1678.776941	219459.377750	36.863360
1680.221048	219859.722624	36.868378
1682.225925	220246.562295	36.873396
1683.826758	220649.321506	36.878413
1685.693513	221024.326079	36.883431
1687.610845	221423.020802	36.888448
1689.536032	221805.536129	36.893466
1690.506346	222181.510611	36.898484
1692.222073	222578.922999	36.903501
1694.026806	222981.096618	36.908519
1695.905576	223374.445195	36.913536
1697.562185	223759.501904	36.918554
1699.141349	224130.730113	36.923572
1700.747079	224510.387670	36.928589
1702.475774	224890.761930	36.933607
1704.367830	225259.349111	36.938624
1705.681994	225641.015711	36.943642
1707.373174	226006.667548	36.948660
1708.797401	226394.743766	36.953677
1710.826719	226776.545280	36.958695
1712.092763	227149.512077	36.963712
1713.899124	227551.217075	36.968730
1715.931651	227925.197848	36.973748
1717.124298	228323.301555	36.978765
1718.351646	228727.471212	36.983783
1720.241946	229117.558109	36.988800
1721.701830	229540.055025	36.993818
1723.591237	229947.823283	36.998836
1724.681049	230374.094385	37.003853
1726.919316	230786.504380	37.008871
1728.798008	231204.438228	37.013888
1730.024522	231626.701350	37.018906
1731.594668	232044.512353	37.023924
1733.252455	232475.314924	37.028941
1734.929640	232914.446953	37.033959
1736.742026	233352.947340	37.038976
1738.112670	233789.949505	37.043994
1740.002338	234233.290562	37.049012
1741.726070	234689.107922	37.054029
1743.001839	235142.818489	37.059047
1745.274466	235586.656111	37.064064
1746.835156	236048.118443	37.069082
1748.838323	236497.643453	37.074100
1751.129921	236959.770313	37.079117
1752.661740	237404.703993	37.084135
1754.832201	237844.398131	37.089152
1756.449263	238308.675509	37.094170
1758.048863	238753.270141	37.099188
1759.837574	239209.213500	37.104205
1761.492539	239670.235690	37.109223
1762.822027	240136.242506	37.114240
1764.388679	240605.689760	37.119258
1766.505817	241069.785406	37.124276
1768.460207	241539.396659	37.129293
1770.277778	242004.612099	37.134311
1772.646410	242465.339404	37.139328
1774.945169	242907.916537	37.144346
1777.598313	243347.207574	37.149364
1779.657869	243770.241460	37.154381
1781.644397	244201.442681	37.159399
1783.653637	244637.670334	37.164416
1785.217918	245066.023598	37.169434
1787.135599	245495.815697	37.174452
1788.527132	245923.183431	37.179469
1789.982857	246353.665221	37.184487
1792.473493	246778.737446	37.189504
1793.911564	247196.470906	37.194522
1796.031574	247600.522944	37.199540
1797.853903	248002.314600	37.204557
1799.422156	248413.752397	37.209575
1801.323207	248808.316815	37.214592
1802.740128	249209.873978	37.219610
1804.769008	249610.336035	37.224628
1806.568704	250008.398884	37.229645
1808.248668	250414.713075	37.234663
1810.539125	250819.856160	37.239680
1812.033981	251233.874251	37.244698
1813.801107	251632.248479	37.249716
1815.740721	252038.519180	37.254733
1817.492599	252446.016134	37.259751
1819.428538	252856.072899	37.264768
1820.848945	253272.492595	37.269786
1822.952006	253682.876723	37.274804
1824.874648	254086.382174	37.279821
1826.484444	254509.628720	37.284839
1828.366113	254914.157509	37.289856
1829.885100	255337.368957	37.294874
1831.513924	255765.870948	37.299892
1833.348207	256203.051138	37.304909
1834.765236	256630.624105	37.309927
1836.842066	257058.287440	37.314944
1838.374728	257502.352703	37.319962
1840.543328	257946.105923	37.324980
1842.116362	258398.598047	37.329997
1843.762509	258845.488880	37.335015
1845.580695	259293.493326	37.340032
1847.251421	259759.660740	37.345050
1849.354159	260210.613807	37.350068
1851.003104	260657.274982	37.355085
1852.834389	261125.472049	37.360103
1854.702941	261590.385501	37.365120
1856.187775	262046.244614	37.370138
1858.265302	262520.495535	37.375156
1860.300634	262993.381588	37.380173
1861.758005	263466.391565	37.385191
1863.676837	263940.033525	37.390208
1865.357938	264418.440716	37.395226
1867.378860	264904.029207	37.400244
1869.012445	265388.591152	37.405261
1870.777644	265881.436853	37.410279
1873.084841	266363.520075	37.415296
1874.669261	266861.450770	37.420314
1876.474400	267356.574185	37.425332
1878.232324	267847.665991	37.430349
1880.035487	268344.160197	37.435367
1881.786873	268848.054761	37.440384
1883.432027	269364.388669	37.445402
1885.464797	269860.053887	37.450420
1887.369553	270366.510928	37.455437
1888.965779	270882.520454	37.460455
1891.262712	271378.264991	37.465472
1892.748685	271887.788498	37.470490
1894.751340	272385.181909	37.475508
1896.353816	272880.788445	37.480525
1897.994529	273373.669420	37.485543
1899.966923	273865.324168	37.490560
1901.773840	274363.356768	37.495578
1903.879364	274875.232219	37.500596
1905.851821	275377.501861	37.505613
1907.298956	275889.487588	37.510631
1908.987204	276397.239516	37.515648
1910.579182	276931.475492	37.520666
1912.290328	277458.729562	37.525684
1913.950345	277983.984226	37.530701
1915.939646	278526.403509	37.535719
1918.008166	279059.205847	37.540736
1920.102486	279600.232334	37.545754
1921.867659	280130.492439	37.550772
1924.211663	280686.637592	37.555789
1925.551542	281234.748041	37.560807
1927.840581	281784.497838	37.565824
1929.779483	282334.661284	37.570842
1931.853378	282882.183434	37.575860
1934.526993	283424.978111	37.580877
1935.753034	283987.678747	37.585895
1938.018999	284528.684926	37.590912
1939.994918	285079.873607	37.595930
1942.429382	285636.798493	37.600948
1944.554335	286180.464253	37.605965
1946.399827	286736.190075	37.610983
1947.993994	287288.324371	37.616000
1949.950717	287850.554458	37.621018
1951.606318	288412.147837	37.626036
1953.759802	288972.282018	37.631053
1955.379238	289553.993345	37.636071
1957.401881	290122.704526	37.641088
1959.055049	290691.603252	37.646106
1960.741637	291275.606276	37.651124
1962.530025	291863.322714	37.656141
1964.480224	292464.698699	37.661159
1966.794013	293044.369297	37.666176
1968.591644	293640.837712	37.671194
1970.798109	294229.333952	37.676212
1973.233824	294806.205998	37.681229
1975.350996	295406.927874	37.686247
1977.676256	295983.558445	37.691264
1979.877679	296561.324524	37.696282
1982.355974	297130.582417	37.701300
1984.887568	297691.573641	37.706317
1986.815693	298264.322529	37.711335
1989.086955	298808.030620	37.716352
1991.509046	299360.675209	37.721370
1993.498761	299918.012885	37.726388
1995.532662	300470.285665	37.731405
1997.198814	301029.780056	37.736423
1998.918138	301584.004790	37.741440
2000.545049	302135.118149	37.746458
2002.177735	302674.925637	37.751476
2004.432190	303216.350473	37.756493
2005.964859	303770.339616	37.761511
2008.073716	304303.351032	37.766528
2010.203178	304846.260060	37.771546
2011.980542	305382.978451	37.776564
2014.840008	305918.289358	37.781581
2016.629754	306458.731881	37.786599
2018.573788	306994.243158	37.791616
2020.782021	307531.153248	37.796634
2022.879519	308073.792568	37.801652
2025.025350	308620.864016	37.806669
2026.379150	309163.089757	37.811687
2028.582463	309710.473891	37.816704
2030.466029	310272.205810	37.821722
2031.949993	310842.483562	37.826740
2033.831161	311400.728542	37.831757
2035.886163	311978.061097	37.836775
2038.011169	312561.446222	37.841792
2039.725661	313129.457757	37.846810
2042.261772	313716.470741	37.851828
2044.518370	314290.728688	37.856845
2046.238302	314866.394182	37.861863
2048.286681	315441.110053	37.866880
2050.679509	316012.562840	37.871898
2052.872818	316598.416917	37.876916
2055.224928	317177.179869	37.881933
2056.980525	317769.776742	37.886951
2058.844210	318349.298698	37.891968
2060.849965	318946.590508	37.896986
2062.796152	319540.129207	37.902004
2065.086615	320126.748118	37.907021
2067.127406	320733.691373	37.912039
2069.308905	321329.915501	37.917056
2071.202694	321929.839362	37.922074
2073.097595	322542.274429	37.927092
2075.059738	323143.774467	37.932109
2077.332464	323753.213120	37.937127
2080.047412	324359.523371	37.942144
2081.637499	324973.941170	37.947162
2083.282156	325585.296709	37.952180
2084.881942	326205.869536	37.957197
2086.940017	326833.999206	37.962215
2089.071918	327464.851342	37.967232
2091.263887	328093.959965	37.972250
2092.871686	328732.554786	37.977268
2095.054190	329367.769239	37.982285
2096.764555	330007.068315	37.987303
2098.951928	330662.424121	37.992320
2100.575133	331313.096065	37.997338
2102.474057	331971.531892	38.002356
2105.034149	332635.913752	38.007373
2106.972534	333298.159831	38.012391
2109.292090	333955.814029	38.017408
2111.785163	334606.576593	38.022426
2113.740155	335251.254759	38.027444
2115.671269	335883.617900	38.032461
2117.913923	336500.588423	38.037479
2120.627878	337127.091112	38.042496
2123.625552	337730.566108	38.047514
2126.169730	338336.649665	38.052532
2129.313767	338923.383589	38.057549
2131.168075	339523.428169	38.062567
2133.945138	340107.926409	38.067584
2136.187206	340685.935388	38.072602
2138.169896	341275.428666	38.077620
2140.332137	341855.391663	38.082637
2142.699070	342449.880970	38.087655
2145.072433	343018.829413	38.092672
2147.191891	343601.798662	38.097690
2148.860109	344192.070964	38.102708
2150.748037	344770.877628	38.107725
2153.037843	345369.860612	38.112743
2154.558377	345965.211321	38.117760
2156.599697	346581.833598	38.122778
2158.122091	347197.089692	38.127796
2159.942139	347806.119781	38.132813
2161.691684	348445.783755	38.137831
2163.574591	349087.344350	38.142848
2165.478857	349727.496271	38.147866
2167.589242	350387.016196	38.152884
2170.024530	351037.106994	38.157901
2171.787943	351682.836863	38.162919
2173.884197	352349.028310	38.167936
2176.228074	353021.256858	38.172954
2178.492687	353684.480520	38.177972
2181.078369	354340.077492	38.182989
2183.699644	355014.332741	38.188007
2185.575242	355669.066001	38.193024
2188.645596	356325.233778	38.198042
2190.881920	356982.421648	38.203060
2193.215172	357633.797605	38.208077
2195.256377	358293.255639	38.213095
2197.080588	358948.883584	38.218112
2199.657741	359619.873260	38.223130
2201.773136	360285.247664	38.228148
2204.300202	360939.174922	38.233165
2206.452814	361599.751205	38.238183
2208.840839	362260.174530	38.243200
2211.059008	362918.180254	38.248218
2213.016352	363598.593594	38.253236
2215.352465	364252.040748	38.258253
2217.980286	364923.843058	38.263271
2219.815135	365585.368748	38.268288
2222.112161	366251.750075	38.273306
2224.412466	366914.517004	38.278324
2226.436752	367573.463759	38.283341
2228.589849	368243.562433	38.288359
2230.658847	368926.827137	38.293376
2232.978610	369584.621788	38.298394
2234.377674	370256.663758	38.303412
2236.426070	370914.937014	38.308429
2238.190381	371578.978541	38.313447
2240.167958	372246.521808	38.318464
2241.631482	372918.502447	38.323482
2243.976473	373600.387707	38.328500
2246.158660	374291.620012	38.333517
2248.170630	374988.041000	38.338535
2250.603726	375692.871227	38.343552
2252.903325	376395.351400	38.348570
2254.877316	377100.408545	38.353588
2257.285775	377794.980087	38.358605
2259.405581	378516.287631	38.363623
2261.676802	379249.040220	38.368640
2263.945127	379964.864714	38.373658
2265.929566	380692.892818	38.378676
2268.074724	381429.447233	38.383693
2270.660077	382166.822516	38.388711
2272.923320	382912.121096	38.393728
2275.241790	383646.846118	38.398746
2277.581376	384400.007312	38.403764
2279.779862	385141.893226	38.408781
2281.857402	385896.863716	38.413799
2284.094285	386659.723630	38.418816
2286.097547	387426.762303	38.423834
2288.665270	388193.001135	38.428852
2290.698884	388974.901807	38.433869
2292.398607	389758.360569	38.438887
2294.801961	390534.429579	38.443904
2297.439222	391322.072982	38.448922
2299.708216	392111.203534	38.453940
2302.542032	392904.094653	38.458957
2304.959634	393684.287408	38.463975
2307.274277	394478.644646	38.468992
2310.040054	395267.302467	38.474010
2312.544838	396052.334338	38.479028
2315.184204	396821.280505	38.484045
2317.861984	397594.634475	38.489063
2320.385423	398378.029041	38.494080
2322.960845	399137.168202	38.499098
2325.443735	399916.371794	38.504116
2327.535428	400681.963297	38.509133
2330.198159	401451.921244	38.514151
2332.498430	402219.639670	38.519168
2335.036660	402978.453820	38.524186
2337.460822	403745.880956	38.529204
2339.685915	404507.316352	38.534221
2342.429460	405273.632927	38.539239
2344.772034	406032.345747	38.544256
2347.837461	406778.576602	38.549274
2350.219283	407532.731449	38.554292
2352.765494	408273.639245	38.559309
2355.728496	409013.771362	38.564327
2357.746704	409749.332992	38.569344
2360.313566	410469.861290	38.574362
2362.421353	411177.403989	38.579380
2365.113338	411873.126113	38.584397
2366.848424	412582.037016	38.589415
2368.800427	413293.880117	38.594432
2371.056247	413995.141359	38.599450
2373.348714	414718.233192	38.604468
2375.298893	415439.311869	38.609485
2377.629414	416165.471303	38.614503
2379.227177	416898.445956	38.619520
2381.453667	417639.395160	38.624538
2382.977694	418388.064540	38.629556
2385.239354	419143.244942	38.634573
2387.523877	419909.387612	38.639591
2389.940500	420685.485291	38.644608
2392.175802	421456.475232	38.649626
2394.583606	422247.362053	38.654644
2396.989960	423037.109637	38.659661
2399.457745	423824.289510	38.664679
2401.449274	424614.613734	38.669696
2404.016924	425417.724063	38.674714
2406.497628	426237.073830	38.679732
2408.301787	427038.336524	38.684749
2410.878544	427869.510852	38.689767
2413.187084	428700.448739	38.694784
2415.427853	429541.088029	38.699802
2417.440025	430394.542754	38.704820
2419.471831	431259.149195	38.709837
2421.860506	432110.755664	38.714855
2423.603319	432986.836559	38.719872
2425.716514	433876.131433	38.724890
2427.491595	434773.445731	38.729908
2429.891723	435673.755432	38.734925
2432.462593	436580.983611	38.739943
2434.491517	437493.631766	38.744960
2437.152407	438417.165688	38.749978
2439.890625	439343.431040	38.754996
2442.470270	440273.175950	38.760013
2445.482381	441201.947639	38.765031
2447.730387	442131.569493	38.770048
2450.407129	443065.226864	38.775066
2452.862862	443999.337159	38.780084
2455.393251	444936.985893	38.785101
2458.105582	445872.741626	38.790119
2460.729700	446810.899393	38.795136
2462.960044	447746.301258	38.800154
2465.649674	448688.158283	38.805172
2468.242518	449617.346113	38.810189
2471.199022	450544.357136	38.815207
2473.873286	451481.539777	38.820224
2476.411215	452407.426802	38.825242
2478.805080	453343.612309	38.830260
2481.045471	454278.719590	38.835277
2483.633989	455205.533777	38.840295
2485.982074	456149.182861	38.845312
2488.945396	457058.203521	38.850330
2491.469663	457966.651598	38.855348
2494.342032	458854.727840	38.860365
2497.406238	459725.191153	38.865383
2499.999160	460600.903295	38.870400
2502.302120	461472.279406	38.875418
2504.725324	462359.567992	38.880436
2507.084462	463241.975548	38.885453
2509.906438	464115.925364	38.890471
2511.924502	465000.434276	38.895488
2513.910313	465890.719705	38.900506
2516.215422	466786.316339	38.905524
2518.832375	467696.269191	38.910541
2521.385398	468598.054915	38.915559
2523.759262	469500.636940	38.920576
2526.174870	470411.252332	38.925594
2529.268278	471326.507283	38.930612
2531.761676	472238.486097	38.935629
2534.410745	473158.981286	38.940647
2537.266180	474084.194342	38.945664
2539.500903	475003.860808	38.950682
2542.269924	475930.713642	38.955700
2544.586975	476856.536416	38.960717
2546.981621	477782.804136	38.965735
2549.194335	478720.670660	38.970752
2551.968017	479658.140381	38.975770
2554.370154	480608.803832	38.980788
2556.692805	481554.230070	38.985805
2559.189162	482506.190716	38.990823
2561.336151	483468.206915	38.995840
2563.828821	484424.760752	39.000858
2566.606989	485402.971001	39.005876
2569.130214	486372.286462	39.010893
2572.471503	487329.698426	39.015911
2575.031027	488306.824981	39.020928
2577.705412	489270.805522	39.025946
2580.239844	490245.707424	39.030964
2582.734422	491220.056347	39.035981
2585.592829	492201.453130	39.040999
2587.749082	493185.840053	39.046016
2590.354209	494162.827858	39.051034
2593.142989	495155.367912	39.056052
2594.922575	496166.687978	39.061069
2597.362852	497160.632325	39.066087
2600.002604	498166.287047	39.071104
2602.447025	499178.774161	39.076122
2604.934165	500188.771190	39.081140
2607.324177	501216.979841	39.086157
2610.072773	502248.744276	39.091175
2612.299699	503281.238769	39.096192
2614.621095	504306.188990	39.101210
2617.371811	505363.068472	39.106228
2619.802130	506411.413055	39.111245
2622.530211	507459.587995	39.116263
2624.849115	508518.804126	39.121280
2627.880472	509553.531892	39.126298
2630.169348	510586.655745	39.131316
2632.616138	511615.955447	39.136333
2635.622754	512628.713043	39.141351
2637.874546	513657.861858	39.146368
2640.812750	514682.743882	39.151386
2643.824492	515700.038040	39.156404
2646.103541	516726.106992	39.161421
2648.875729	517753.131775	39.166439
2651.851750	518802.269420	39.171456
2654.280717	519823.672566	39.176474
2657.044570	520861.975211	39.181492
2659.645966	521906.882975	39.186509
2662.530281	522948.094306	39.191527
2665.137291	523985.806109	39.196544
2668.493314	525034.195056	39.201562
2671.200200	526067.867830	39.206580
2674.094492	527106.370935	39.211597
2677.341335	528138.346999	39.216615
2679.701796	529176.946790	39.221632
2681.753561	530224.788225	39.226650
2684.857187	531269.455429	39.231668
2687.509829	532319.761911	39.236685
2690.590887	533364.081125	39.241703
2693.726484	534414.052521	39.246720
2696.259554	535461.332969	39.251738
2699.551886	536497.488420	39.256756
2701.961452	537545.643782	39.261773
2704.664483	538581.698112	39.266791
2708.079247	539619.919473	39.271808
2710.638701	540667.617127	39.276826
2714.062519	541693.812800	39.281844
2716.562595	542725.120614	39.286861
2719.499679	543764.977916	39.291879
2722.415354	544799.531233	39.296896
2724.723558	545836.273272	39.301914
2727.294259	546871.183077	39.306932
2729.810619	547928.899813	39.311949
2732.337202	548976.730089	39.316967
2734.719672	550031.994485	39.321984
2737.133357	551099.486366	39.327002
2739.940655	552165.670872	39.332020
2742.403570	553245.147852	39.337037
2745.015650	554326.924751	39.342055
2747.619351	555407.510220	39.347072
2750.186608	556500.675850	39.352090
2753.054918	557589.228760	39.357108
2755.547064	558695.489594	39.362125
2758.120401	559798.378701	39.367143
2760.907117	560914.499167	39.372160
2763.108328	562041.372141	39.377178
2765.988440	563169.036068	39.382196
2768.101569	564304.415835	39.387213
2770.387145	565438.361022	39.392231
2773.256226	566591.937751	39.397248
2775.492102	567740.900492	39.402266
2778.722346	568862.333553	39.407284
2781.148610	569987.017462	39.412301
2783.740067	571107.156946	39.417319
2786.764107	572245.289421	39.422336
2789.481438	573374.590187	39.427354
2792.229395	574501.777073	39.432372
2794.840494	575655.073965	39.437389
2797.137661	576806.862854	39.442407
2799.809232	577976.437995	39.447424
2802.014652	579156.564724	39.452442
2804.913299	580341.876044	39.457460
2807.489574	581530.487523	39.462477
2810.140586	582721.978927	39.467495
2812.927930	583935.490131	39.472512
2815.356276	585151.046559	39.477530
2818.106217	586365.022077	39.482548
2820.936365	587610.988242	39.487565
2823.677624	588851.477607	39.492583
2826.721868	590090.182626	39.497600
2829.155983	591346.198759	39.502618
2832.540714	592596.157730	39.507636
2835.684384	593854.240595	39.512653
2838.351543	595118.280551	39.517671
2841.445096	596379.055896	39.522688
2844.437267	597641.414626	39.527706
2847.635942	598896.590558	39.532724
2850.812903	600174.063538	39.537741
2853.794962	601435.508576	39.542759
2856.924982	602692.334523	39.547776
2859.846325	603956.915537	39.552794
2862.845158	605218.640256	39.557812
2865.607238	606490.973120	39.562829
2867.972057	607759.577937	39.567847
2871.488712	609032.995597	39.572864
2874.039790	610320.989599	39.577882
2877.006530	611597.410229	39.582900
2879.754910	612878.322391	39.587917
2882.595798	614163.220807	39.592935
2886.000223	615452.523003	39.597952
2889.021397	616740.239457	39.602970
2892.188751	618015.682539	39.607988
2895.100129	619305.114595	39.613005
2898.108616	620587.030565	39.618023
2901.182399	621864.436085	39.623040
2903.868367	623151.649010	39.628058
2907.058485	624427.331129	39.633076
2910.267867	625711.349376	39.638093
2913.239455	626996.402151	39.643111
2915.968562	628270.054503	39.648128
2918.442385	629551.686129	39.653146
2921.731672	630839.662755	39.658164
2924.374089	632136.976821	39.663181
2927.479233	633413.735674	39.668199
2930.850216	634710.355704	39.673216
2933.534250	635991.112079	39.678234
2936.544305	637239.570994	39.683252
2939.369682	638505.770723	39.688269
2942.361397	639743.850906	39.693287
2945.149148	640983.013111	39.698304
2947.510933	642223.244460	39.703322
2950.469942	643465.964963	39.708340
2953.511476	644725.919706	39.713357
2956.326816	645977.679445	39.718375
2959.062447	647243.602950	39.723392
2962.151618	648513.692003	39.728410
2965.164875	649774.961191	39.733428
2968.482582	651045.186717	39.738445
2971.032084	652319.266679	39.743463
2974.136422	653598.716571	39.748480
2976.760951	654886.200813	39.753498
2980.302712	656168.827340	39.758516
2983.249134	657459.802552	39.763533
2985.765355	658755.509554	39.768551
2989.021580	660060.176567	39.773568
2991.591422	661376.681001	39.778586
2994.438812	662677.878256	39.783604
2997.311913	664015.718335	39.788621
3000.132501	665346.016553	39.793639
3003.025592	666677.211127	39.798656
3005.577212	668030.262749	39.803674
3008.563284	669386.428548	39.808692
3011.555818	670752.442834	39.813709
3013.842310	672131.604275	39.818727
3017.209716	673514.354793	39.823744
3019.498620	674921.936475	39.828762
3022.733505	676319.551906	39.833780
3025.287661	677738.438787	39.838797
3027.842915	679154.126287	39.843815
3031.448926	680581.834565	39.848832
3034.233185	682023.118522	39.853850
3037.204654	683458.829302	39.858868
3040.481709	684911.439859	39.863885
3043.301785	686355.754012	39.868903
3046.774890	687804.539765	39.873920
3049.844996	689268.693556	39.878938
3053.516822	690710.623565	39.883956
3056.874042	692165.173387	39.888973
3059.498134	693622.834314	39.893991
3063.061840	695077.962163	39.899008
3066.566685	696536.479595	39.904026
3069.421947	697990.949186	39.909044
3072.312722	699443.485660	39.914061
3075.587578	700901.860072	39.919079
3079.040812	702362.288138	39.924096
3081.991770	703822.654640	39.929114
3084.928758	705277.277818	39.934132
3088.100638	706734.932942	39.939149
3091.174983	708199.833827	39.944167
3094.419592	709650.442745	39.949184
3097.555921	711089.734216	39.954202
3100.983504	712509.874415	39.959220
3104.642079	713920.136082	39.964237
3107.514577	715318.322110	39.969255
3110.431995	716706.521920	39.974272
3113.440631	718106.098612	39.979290
3116.766314	719496.979007	39.984308
3120.032367	720903.112234	39.989325
3123.187726	722303.834502	39.994343
3125.822977	723696.103752	39.999360
3128.963911	725111.425500	40.004378
3132.226152	726516.995071	40.009396
3135.310533	727929.664153	40.014413
3138.173597	729354.029122	40.019431
3141.521005	730774.900357	40.024448
3144.520988	732209.948988	40.029466
3147.403774	733637.998474	40.034484
3150.993314	735079.690444	40.039501
3153.719357	736520.381442	40.044519
3156.831246	737974.955698	40.049536
3159.538493	739424.794026	40.054554
3163.095596	740889.461745	40.059572
3165.960068	742358.660161	40.064589
3168.600829	743841.476048	40.069607
3171.847837	745328.442492	40.074624
3174.695500	746823.769033	40.079642
3178.144089	748316.044449	40.084660
3181.405587	749820.873141	40.089677
3183.997813	751339.658946	40.094695
3187.325564	752861.318688	40.099712
3189.874506	754397.678414	40.104730
3193.478341	755930.398500	40.109748
3196.877977	757473.229200	40.114765
3200.036679	759026.415497	40.119783
3203.275425	760560.771334	40.124800
3206.447704	762123.304154	40.129818
3209.685765	763681.123707	40.134836
3212.680833	765241.954143	40.139853
3216.508986	766812.539392	40.144871
3219.552825	768388.381153	40.149888
3222.424871	769959.691002	40.154906
3225.537610	771538.926516	40.159924
3228.840708	773120.245510	40.164941
3231.739431	774713.419909	40.169959
3235.170629	776299.724355	40.174976
3238.453636	777907.008490	40.179994
3241.380039	779500.011910	40.185012
3245.049784	781098.178314	40.190029
3248.298954	782714.453892	40.195047
3251.534530	784316.587820	40.200064
3254.645261	785934.610714	40.205082
3257.895915	787552.633647	40.210100
3260.621373	789165.966492	40.215117
3263.568046	790804.760444	40.220135
3267.334523	792424.959006	40.225152
3271.103114	794034.303330	40.230170
3274.399244	795629.110800	40.235188
3278.287513	797195.356423	40.240205
3281.597167	798764.430065	40.245223
3284.699479	800312.977123	40.250240
3288.009191	801869.847304	40.255258
3291.225387	803434.547116	40.260276
3294.563470	804996.961567	40.265293
3298.071385	806555.860733	40.270311
3301.199040	808132.206575	40.275328
3303.881617	809707.773000	40.280346
3307.234499	811297.217940	40.285364
3310.818137	812881.511042	40.290381
3313.960476	814480.151878	40.295399
3317.326248	816059.628718	40.300416
3320.799714	817650.863567	40.305434
3324.004414	819253.910865	40.310452
3327.389280	820854.782960	40.315469
3330.511992	822467.209366	40.320487
3333.999776	824080.055211	40.325504
3337.372190	825699.249473	40.330522
3340.108110	827318.589103	40.335540
3343.854294	828957.813425	40.340557
3347.146206	830588.518496	40.345575
3350.792466	832231.069989	40.350592
3354.234850	833869.245413	40.355610
3357.109129	835522.575035	40.360628
3360.566701	837168.030812	40.365645
3363.488724	838835.381546	40.370663
3366.820124	840500.716973	40.375680
3370.142357	842177.477468	40.380698
3373.304367	843866.844491	40.385716
3377.136752	845546.993971	40.390733
3379.896626	847244.071201	40.395751
3383.585833	848936.934497	40.400768
3386.786705	850646.606346	40.405786
3389.973495	852353.284869	40.410804
3393.222739	854068.894069	40.415821
3396.799440	855801.043710	40.420839
3400.013986	857523.842638	40.425856
3403.542410	859253.761962	40.430874
3406.875795	860989.620449	40.435892
3410.405736	862726.692806	40.440909
3413.382529	864475.857488	40.445927
3416.487397	866224.589077	40.450944
3419.963096	867991.434206	40.455962
3423.120114	869759.650641	40.460980
3426.562975	871528.261109	40.465997
3429.869783	873309.330295	40.471015
3433.503149	875093.095414	40.476032
3437.065754	876869.372047	40.481050
3439.983733	878659.138573	40.486068
3443.753526	880442.608538	40.491085
3447.416171	882242.067681	40.496103
3451.104586	884035.944087	40.501120
3454.397184	885805.537746	40.506125
3457.786309	887532.514806	40.511130
3461.712550	889194.854674	40.516135
3464.927624	890790.890963	40.521140
3468.357742	892308.629820	40.526144
3471.776077	893749.137505	40.531149
3475.109313	895110.261873	40.536154
3478.918543	896391.093980	40.541159
3481.787152	897590.190982	40.546164
3484.580418	898698.670139	40.551168
3487.551940	899730.249588	40.556173
3490.120991	900684.105162	40.561178
3492.462354	901555.903597	40.566183
3494.663383	902372.010599	40.571188
3497.012385	903112.236937	40.576192
3499.269763	903786.782698	40.581197
3500.964606	904392.665374	40.586202
3502.934568	904928.028282	40.591207
3504.806053	905402.503071	40.596212
3506.403131	905835.518301	40.601216
3508.119258	906208.309897	40.606221
3509.814751	906521.395933	40.611226
3511.568345	906780.847300	40.616231
3512.814657	907010.581853	40.621236
3514.229723	907178.094556	40.626240
3515.637975	907292.772524	40.631245
3516.371024	907378.448961	40.636250
3517.771556	907420.724536	40.641255
3518.635371	907437.255050	40.646260
3519.892372	907408.311817	40.651264
3520.740246	907350.805758	40.656269
3521.310757	907261.821263	40.661274
3522.325934	907140.365876	40.666279
3522.711576	907003.492969	40.671284
3523.561292	906837.805882	40.676288
3524.392929	906645.505544	40.681293
3524.739631	906436.696768	40.686298
3525.640669	906202.425520	40.691303
3525.861798	905952.445886	40.696308
3526.457110	905668.445996	40.701312
3527.170623	905373.610087	40.706317
3527.644375	905084.586187	40.711322
3528.610607	904755.146761	40.716327
3528.487095	904416.517521	40.721332
3528.535786	904065.105150	40.726336
3529.285665	903706.990993	40.731341
3529.138304	903326.914046	40.736346
3529.852129	902941.261155	40.741351
3530.022543	902555.674376	40.746356
3530.339840	902136.744711	40.751360
3530.637953	901725.603709	40.756365
3530.644868	901298.364886	40.761370
3531.081230	900874.494797	40.766375
3530.899174	900438.632495	40.771380
3531.343962	899988.245823	40.776384
3531.838408	899537.911071	40.781389
3531.468607	899071.274391	40.786394
3531.750825	898614.819279	40.791399
3532.044614	898135.922055	40.796404
3532.096352	897656.156264	40.801408
3532.196667	897172.188327	40.806413
3532.542993	896698.472013	40.811418
3532.869755	896197.768394	40.816423
3532.575291	895699.155219	40.821428
3532.532388	895202.387463	40.826432
3532.935703	894695.354440	40.831437
3532.745860	894179.970274	40.836442
3533.186054	893668.780625	40.841447
3532.904192	893152.062522	40.846452
3533.340227	892636.044846	40.851456
3533.570322	892121.078905	40.856461
3533.128546	891595.256648	40.861466
3533.544595	891059.764267	40.866471
3533.405070	890528.377702	40.871476
3533.559862	889994.280488	40.876480
3533.659938	889466.815956	40.881485
3533.293934	888930.290566	40.886490
3533.552609	888385.773124	40.891495
3533.611751	887855.845853	40.896500
3533.807809	887306.690032	40.901504
3533.922299	886751.496692	40.906509
3533.401172	886209.421979	40.911514
3533.722342	885654.668290	40.916519
3533.687171	885104.955000	40.921524
3534.109273	884547.851697	40.926528
3533.973211	883996.501512	40.931533
3533.894178	883444.508208	40.936538
3534.212173	882877.871081	40.941543
3534.166361	882321.698679	40.946548
3533.906689	881750.111656	40.951552
3534.046658	881189.053916	40.956557
3534.050509	880626.706169	40.961562
3534.167986	880060.119362	40.966567
3534.126103	879507.164777	40.971572
3534.404505	878934.725436	40.976576
3534.359772	878366.451874	40.981581
3533.996171	877791.297146	40.986586
3534.299128	877212.095508	40.991591
3534.257530	876638.420379	40.996596
3533.985366	876059.590976	41.001600
3534.345110	875485.347101	41.006605
3533.932594	874917.868993	41.011610
3533.855656	874339.806800	41.016615
3533.979093	873762.235646	41.021620
3534.054922	873191.986939	41.026624
3534.212002	872613.522005	41.031629
3534.068070	872038.447063	41.036634
3534.210351	871453.275277	41.041639
3534.359896	870866.589268	41.046644
3534.087790	870284.089683	41.051648
3534.132809	869696.044679	41.056653
3533.860746	869122.650341	41.061658
3534.332403	868531.700295	41.066663
3533.826489	867946.682822	41.071668
3533.680369	867367.080164	41.076672
3533.897860	866786.776800	41.081677
3534.058959	866204.193656	41.086682
3534.177331	865614.666676	41.091687
3534.244936	865035.287739	41.096692
3533.784903	864431.176006	41.101696
3533.724629	863832.472161	41.106701
3533.666228	863248.280323	41.111706
3533.978231	862653.087430	41.116711
3533.920845	862073.250913	41.121716
3533.781853	861475.007013	41.126720
3533.710058	860890.492555	41.131725
3533.717359	860306.588623	41.136730
3533.673445	859712.236729	41.141735
3533.494036	859133.014804	41.146740
3533.748564	858528.678055	41.151744
3533.980671	857928.855050	41.156749
3533.686523	857355.901037	41.161754
3534.072965	856755.936502	41.166759
3533.953474	856161.543233	41.171764
3533.689021	855568.478778	41.176768
3533.677100	854968.212627	41.181773
3533.892216	854381.371878	41.186778
3533.461688	853783.007128	41.191783
3533.413753	853195.417084	41.196788
3533.645903	852598.478323	41.201792
3533.758432	852002.767454	41.206797
3533.761352	851413.733861	41.211802
3533.767591	850805.272411	41.216807
3533.684056	850207.475265	41.221812
3533.906495	849597.105956	41.226816
3533.740121	849006.996238	41.231821
3533.588006	848413.614511	41.236826
3533.866414	847808.123780	41.241831
3533.771560	847210.137684	41.246836
3533.586473	846606.167756	41.251840
3533.793900	846004.800132	41.256845
3533.544441	845416.215657	41.261850
3533.447090	844806.308747	41.266855
3533.525371	844203.913320	41.271860
3533.583279	843606.531248	41.276864
3533.526584	842998.195940	41.281869
3533.534674	842407.238609	41.286874
3533.716677	841786.463809	41.291879
3533.701851	841189.644768	41.296884
3533.490581	840579.542621	41.301888
3533.337208	839972.053305	41.306893
3532.984342	839383.068682	41.311898
3533.021059	838782.454351	41.316903
3533.354101	838177.977377	41.321908
3533.345097	837574.964550	41.326912
3533.793759	836972.694491	41.331917
3533.004100	836368.042187	41.336922
3533.270469	835759.200474	41.341927
3533.224418	835150.793221	41.346932
3533.025747	834547.477872	41.351936
3533.390981	833942.008561	41.356941
3533.377537	833341.476196	41.361946
3533.128875	832738.633712	41.366951
3533.109877	832137.355226	41.371956
3532.988200	831519.829823	41.376960
3533.049622	830915.836138	41.381965
3533.166583	830315.731633	41.386970
3533.263956	829706.686987	41.391975
3532.974422	829095.746368	41.396980
3532.877885	828485.301309	41.401984
3532.976351	827880.822636	41.406989
3532.841713	827284.583531	41.411994
3533.223420	826676.085169	41.416999
3533.003277	826079.799152	41.422004
3532.746777	825467.583451	41.427008
3532.883909	824853.288330	41.432013
3532.683961	824249.647767	41.437018
3532.751719	823643.266350	41.442023
3532.610432	823039.113182	41.447028
3532.409079	822436.625743	41.452032
3532.688665	821839.183603	41.457037
3532.622513	821242.284114	41.462042
3532.749543	820628.573165	41.467047
3532.241744	820031.248198	41.472052
3532.534949	819426.591500	41.477056
3532.518808	818813.812412	41.482061
3532.199075	818227.396147	41.487066
3532.716475	817616.861277	41.492071
3532.696004	817007.047095	41.497076
3532.729955	816403.137513	41.502080
3532.578488	815792.500359	41.507085
3532.248630	815188.053336	41.512090
3532.554883	814582.610880	41.517095
3532.163443	813980.169726	41.522100
3532.026515	813381.547283	41.527104
3532.453034	812762.750688	41.532109
3532.256123	812168.289642	41.537114
3532.490312	811556.514479	41.542119
3532.254727	810952.256722	41.547124
3532.083598	810342.301351	41.552128
3532.188196	809740.668584	41.557133
3531.886216	809138.512772	41.562138
3532.336634	808535.538006	41.567143
3532.233171	807927.459647	41.572148
3532.319723	807315.864355	41.577152
3532.390949	806709.165938	41.582157
3531.990035	806105.728484	41.587162
3532.237893	805491.246028	41.592167
3532.322717	804883.255225	41.597172
3532.005508	804288.808685	41.602176
3532.112085	803673.059129	41.607181
3532.025973	803067.828450	41.612186
3532.160186	802452.748897	41.617191
3532.079641	801841.377781	41.622196
3531.930024	801236.486732	41.627200
3531.866945	800631.380562	41.632205
3531.549002	800025.627059	41.637210
3531.558149	799412.209907	41.642215
3531.303887	798817.965720	41.647220
3531.414493	798220.664309	41.652224
3531.475495	797618.020435	41.657229
3531.393872	797021.384467	41.662234
3531.629139	796415.514794	41.667239
3530.974476	795823.536061	41.672244
3531.143036	795224.494466	41.677248
3531.315119	794626.333479	41.682253
3531.105548	794035.403161	41.687258
3531.265365	793436.847807	41.692263
3531.394112	792838.246548	41.697268
3531.350504	792235.400411	41.702272
3531.468695	791631.197962	41.707277
3531.351518	791037.396062	41.712282
3531.374965	790432.762959	41.717287
3531.366604	789836.729055	41.722292
3531.367520	789242.018749	41.727296
3531.796255	788632.298475	41.732301
3531.259281	788026.965298	41.737306
3531.490765	787410.146965	41.742311
3531.509232	786810.118665	41.747316
3531.479123	786198.940406	41.752320
3531.148577	785598.918521	41.757325
3531.099886	784989.064896	41.762330
3531.132796	784383.520481	41.767335
3531.030703	783785.863312	41.772340
3530.866524	783178.873778	41.777344
3530.964314	782583.343770	41.782349
3530.760609	781987.815737	41.787354
3530.820315	781380.291374	41.792359
3530.904520	780793.566173	41.797364
3530.842434	780190.929843	41.802368
3531.231559	779587.231389	41.807373
3530.902212	778989.016842	41.812378
3530.862555	778383.815011	41.817383
3530.926865	777785.679675	41.822388
3530.832262	777187.817332	41.827392
3530.980680	776577.757513	41.832397
3530.995339	775978.940290	41.837402
3531.139570	775368.681261	41.842407
3530.914695	774760.747752	41.847412
3530.872621	774159.870788	41.852416
3530.843369	773552.984791	41.857421
3530.855920	772952.786994	41.862426
3530.744852	772341.924653	41.867431
3530.788580	771737.682568	41.872436
3530.198433	771144.284914	41.877440
3530.641515	770537.364141	41.882445
3530.698706	769944.793574	41.887450
3530.471125	769346.213917	41.892455
3530.355782	768743.477400	41.897460
3530.026958	768150.730167	41.902464
3530.161775	767549.183936	41.907469
3530.381163	766966.743902	41.912474
3530.403750	766362.804514	41.917479
3530.680113	765767.989341	41.922484
3530.106848	765169.328423	41.927488
3530.431513	764563.170503	41.932493
3530.243010	763971.495449	41.937498
3530.268342	763371.257007	41.942503
3530.294185	762769.589747	41.947508
3529.953793	762171.487046	41.952512
3530.268284	761572.238575	41.957517
3529.814118	760979.978092	41.962522
3529.996086	760379.966770	41.967527
3530.019204	759789.306735	41.972532
3529.990208	759187.954089	41.977536
3530.162095	758592.094008	41.982541
3529.868113	758004.505923	41.987546
3529.733504	757409.394475	41.992551
3529.957781	756816.938412	41.997556
3529.716735	756228.660917	42.002560
3529.874285	755629.658963	42.007565
3529.861605	755045.149905	42.012570
3530.006750	754441.713311	42.017575
3529.754093	753850.095105	42.022580
3529.734056	753253.503941	42.027584
3529.557932	752655.214292	42.032589
3529.360753	752064.287980	42.037594
3529.670225	751474.612339	42.042599
3529.720297	750888.935852	42.047604
3529.318936	750295.241737	42.052608
3529.670836	749692.976794	42.057613
3529.130612	749115.662914	42.062618
3529.305049	748528.057179	42.067623
3529.343248	747935.835681	42.072628
3528.948221	747349.571664	42.077632
3529.341088	746757.545536	42.082637
3529.061708	746176.015405	42.087642
3529.356583	745586.535845	42.092647
3529.462313	744999.317389	42.097652
3529.287313	744410.471672	42.102656
3529.288988	743813.395712	42.107661
3529.101720	743237.908422	42.112666
3529.163116	742645.231581	42.117671
3529.356892	742062.029269	42.122676
3529.207169	741473.502452	42.127680
3528.842322	740891.594268	42.132685
3528.955290	740307.484622	42.137690
3528.542021	739719.119062	42.142695
3528.789614	739141.081990	42.147700
3528.796220	738565.665321	42.152704
3528.992027	737979.391161	42.157709
3528.569537	737394.861199	42.162714
3528.506044	736800.678750	42.167719
3528.612686	736223.541680	42.172724
3528.318001	735651.824631	42.177728
3528.493441	735070.238155	42.182733
3528.722423	734494.885063	42.187738
3528.478737	733918.532009	42.192743
3528.327424	733346.180241	42.197748
3528.504829	732765.217959	42.202752
3528.578190	732190.419087	42.207757
3528.439017	731613.090710	42.212762
3528.248982	731024.491285	42.217767
3528.433506	730456.629457	42.222772
3528.250452	729875.124269	42.227776
3528.284523	729299.333930	42.232781
3527.849600	728716.996272	42.237786
3528.278009	728145.711811	42.242791
3527.929481	727581.008176	42.247796
3528.139228	727009.284985	42.252800
3528.131325	726430.029328	42.257805
3527.981935	725863.290269	42.262810
3527.848542	725286.055551	42.267815
3528.089312	724722.292027	42.272820
3527.751032	724152.543464	42.277824
3527.971996	723568.735305	42.282829
3527.689842	723005.884646	42.287834
3527.712366	722436.153686	42.292839
3527.706523	721874.070569	42.297844
3527.683397	721307.094523	42.302848
3527.740342	720739.520623	42.307853
3527.854761	720179.086205	42.312858
3527.770019	719605.361144	42.317863
3527.900910	719034.038634	42.322868
3527.785876	718472.189404	42.327872
3528.015963	717883.069305	42.332877
3527.924543	717330.263107	42.337882
3527.784039	716751.391633	42.342887
3527.751785	716187.787285	42.347892
3527.484307	715613.520883	42.352896
3527.866742	715038.608115	42.357901
3527.498267	714480.948483	42.362906
3527.714573	713909.112031	42.367911
3527.760975	713332.006574	42.372916
3527.733458	712767.774879	42.377920
3527.821024	712194.057758	42.382925
3527.298079	711628.693223	42.387930
3527.647180	711057.831830	42.392935
3527.791638	710489.845533	42.397940
3527.445143	709924.088953	42.402944
3528.078486	709344.576256	42.407949
3527.388403	708780.887050	42.412954
3527.434204	708209.935734	42.417959
3527.405749	707637.320509	42.422964
3526.547794	707076.426906	42.427968
3526.734828	706512.636778	42.432973
3526.951279	705966.433009	42.437978
3526.767173	705403.278855	42.442983
3526.633591	704853.538129	42.447988
3526.723322	704305.015501	42.452992
3526.828070	703731.123462	42.457997
3526.796094	703178.576313	42.463002
3526.666416	702625.215678	42.468007
3526.700988	702073.580091	42.473012
3526.870951	701523.227716	42.478016
3526.649665	700970.621657	42.483021
3526.028871	700417.154238	42.488026
3526.396948	699866.613418	42.493031
3526.443195	699314.303711	42.498036
3526.227964	698766.923876	42.503040
3526.296628	698208.129204	42.508045
3526.109688	697677.425917	42.513050
3526.161671	697124.281004	42.518055
3526.434514	696584.237020	42.523060
3526.291254	696036.425722	42.528064
3526.410923	695487.043897	42.533069
3526.192711	694938.630190	42.538074
3526.111121	694396.175627	42.543079
3526.331889	693845.729585	42.548084
3526.106315	693300.298482	42.553088
3526.053404	692750.378089	42.558093
3526.063736	692215.532535	42.563098
3526.076906	691664.936793	42.568103
3526.235635	691116.570258	42.573108
3525.897529	690570.891282	42.578112
3526.017333	690021.966614	42.583117
3525.633832	689487.173723	42.588122
3526.091462	688941.607628	42.593127
3525.777088	688396.289386	42.598132
3525.759234	687853.126577	42.603136
3525.853771	687310.757714	42.608141
3525.560283	686779.271420	42.613146
3525.804841	686242.834309	42.618151
3525.471497	685704.025132	42.623156
3525.771656	685162.835783	42.628160
3525.886725	684630.904369	42.633165
3525.637361	684092.432859	42.638170
3525.584479	683554.592811	42.643175
3525.888163	683011.332855	42.648180
3525.901413	682478.296952	42.653184
3525.674327	681930.283282	42.658189
3525.655609	681391.712098	42.663194
3525.740446	680851.946114	42.668199
3525.726637	680305.939927	42.673204
3525.517303	679775.523396	42.678208
3525.701611	679233.553291	42.683213
3525.530019	678697.639028	42.688218
3525.718071	678150.324536	42.693223
3525.604508	677607.612119	42.698228
3524.965813	677077.462026	42.703232
3524.755471	676535.500208	42.708237
3524.978908	676016.352020	42.713242
3525.032231	675493.267408	42.718247
3525.086227	674963.276592	42.723252
3524.695361	674438.065653	42.728256
3525.022580	673905.924755	42.733261
3524.650356	673388.126811	42.738266
3524.480713	672862.689605	42.743271
3524.745760	672338.394745	42.748276
3524.897637	671819.074554	42.753280
3525.091285	671294.035546	42.758285
3524.564486	670775.919988	42.763290
3524.925917	670250.494861	42.768295
3525.100168	669721.482549	42.773300
3524.582401	669198.192989	42.778304
3524.709744	668658.807794	42.783309
3524.190107	668154.059917	42.788314
3524.360499	667635.802312	42.793319
3524.597834	667113.265799	42.798324
3524.441837	666590.717786	42.803329
3524.587714	666070.683126	42.808333
3524.645175	665551.483103	42.813338
3524.358129	665033.859974	42.818343
3524.359399	664512.467988	42.823348
3524.315894	664005.273396	42.828353
3524.210786	663479.552833	42.833357
3524.154665	662966.617775	42.838362
3524.006101	662449.829042	42.843367
3524.179482	661947.328497	42.848372
3523.894189	661448.323231	42.853377
3523.801978	660924.656306	42.858381
3523.997243	660408.298123	42.863386
3524.132367	659903.252115	42.868391
3524.272583	659393.437204	42.873396
3523.911852	658870.054199	42.878401
3524.083816	658358.582164	42.883405
3523.684422	657862.056973	42.888410
3523.866370	657356.720623	42.893415
3524.115839	656847.202726	42.898420
3523.768816	656335.113870	42.903425
3523.753734	655823.141214	42.908429
3523.895908	655327.043603	42.913434
3523.796066	654812.336160	42.918439
3524.132331	654295.929225	42.923444
3523.673958	653795.561984	42.928449
3523.530653	653289.471878	42.933453
3523.474276	652780.543946	42.938458
3523.379728	652273.194628	42.943463
3523.573221	651769.666270	42.948468
3523.523042	651277.843052	42.953473
3523.665707	650768.577729	42.958477
3523.660483	650276.347452	42.963482
3523.661492	649764.207138	42.968487
3523.542225	649257.357159	42.973492
3523.130537	648771.317304	42.978497
3523.691938	648268.997689	42.983501
3523.350231	647767.856401	42.988506
3523.342692	647266.383078	42.993511
3522.978502	646768.893665	42.998516
3523.109205	646260.749555	43.003521
3523.086459	645771.198980	43.008525
3523.211586	645278.700278	43.013530
3523.289349	644778.487714	43.018535
3522.995230	644289.311330	43.023540
3522.933164	643796.872207	43.028545
3522.931702	643298.299554	43.033549
3522.909619	642816.254527	43.038554
3522.598939	642329.286031	43.043559
3522.811723	641831.204659	43.048564
3522.581284	641351.525713	43.053569
3522.745661	640853.854803	43.058573
3522.055520	640379.609181	43.063578
3522.446555	639888.803602	43.068583
3522.413447	639412.350492	43.073588
3522.062027	638937.079899	43.078593
3522.361907	638447.021025	43.083597
3522.390070	637986.646778	43.088602
3522.027016	637501.207751	43.093607
3522.301809	637026.592238	43.098612
3522.304025	636539.794945	43.103617
3522.351998	636059.220498	43.108621
3522.061766	635588.387502	43.113626
3522.159819	635120.568869	43.118631
3522.205180	634640.029053	43.123636
3521.813984	634170.750040	43.128641
3522.324721	633691.537998	43.133645
3521.858660	633221.878671	43.138650
3521.995888	632743.437421	43.143655
3521.782432	632271.740427	43.148660
3521.828979	631805.433131	43.153665
3521.940046	631331.636358	43.158669
3521.648612	630867.547274	43.163674
3521.816369	630399.104503	43.168679
3521.848676	629923.305406	43.173684
3521.578409	629459.200561	43.178689
3521.658358	628984.151862	43.183693
3521.689526	628532.320253	43.188698
3521.801015	628065.735883	43.193703
3521.706569	627583.143896	43.198708
3521.185433	627115.524125	43.203713
3521.547512	626643.076080	43.208717
3521.342452	626192.687229	43.213722
3521.487967	625725.242968	43.218727
3521.479378	625263.012863	43.223732
3520.999912	624800.292210	43.228737
3521.217021	624348.651543	43.233741
3521.078211	623895.349623	43.238746
3521.176845	623431.569486	43.243751
3521.180181	622969.588843	43.248756
3521.014511	622527.554264	43.253761
3521.209511	622068.858414	43.258765
3521.130388	621617.353752	43.263770
3520.612958	621159.842975	43.268775
3520.940728	620701.767692	43.273780
3520.836657	620263.537689	43.278785
3520.957222	619808.065332	43.283789
3521.326017	619358.143537	43.288794
3520.818584	618906.097747	43.293799
3520.943845	618465.751556	43.298804
3520.768262	618012.910411	43.303809
3520.896742	617549.373913	43.308813
3520.561302	617118.974951	43.313818
3520.291887	616671.607149	43.318823
3520.332493	616219.556876	43.323828
3520.573452	615780.185315	43.328833
3520.443524	615338.954684	43.333837
3521.049141	614906.954736	43.338842
3520.979212	614450.689852	43.343847
3520.825950	614006.552329	43.348852
3520.164862	613566.594635	43.353857
3520.357278	613115.744506	43.358861
3520.065376	612688.724277	43.363866
3519.917858	612242.760033	43.368871
3520.179272	611807.388350	43.373876
3520.130471	611380.928095	43.378881
3519.947740	610952.017182	43.383885
3519.966444	610517.789798	43.388890
3520.066294	610093.060153	43.393895
3520.065463	609644.609642	43.398900
3520.082081	609220.412694	43.403905
3520.138153	608783.854584	43.408909
3519.984403	608355.842120	43.413914
3519.750170	607921.908217	43.418919
3519.809776	607491.117731	43.423924
3519.468576	607070.462058	43.428929
3519.801225	606643.906598	43.433933
3519.971721	606223.984782	43.438938
3519.720786	605786.911261	43.443943
3520.075395	605356.189541	43.448948
3519.223237	604948.737064	43.453953
3519.457000	604517.000616	43.458957
3519.492160	604099.381328	43.463962
3519.257383	603677.075996	43.468967
3519.578752	603256.165455	43.473972
3519.223658	602849.706993	43.478977
3519.474786	602423.709315	43.483981
3519.409071	602002.617890	43.488986
3519.200302	601591.271819	43.493991
3519.492662	601168.532760	43.498996
3519.082011	600760.252897	43.504001
3519.390212	600336.075117	43.509005
3519.536791	599918.384455	43.514010
3519.196025	599498.402593	43.519015
3519.200317	599085.374337	43.524020
3518.791631	598677.723063	43.529025
3519.010800	598264.829586	43.534029
3519.086087	597862.940628	43.539034
3519.014047	597442.938602	43.544039
3518.998934	597033.154007	43.549044
3518.876616	596621.967400	43.554049
3518.953148	596203.150425	43.559053
3518.565783	595803.428298	43.564058
3518.480531	595412.277800	43.569063
3519.012841	595008.906638	43.574068
3518.985889	594605.617052	43.579073
3519.071448	594196.669749	43.584077
3518.836759	593786.356654	43.589082
3518.714487	593374.453099	43.594087
3518.907885	592965.946743	43.599092
3518.589567	592577.051785	43.604097
3518.423941	592167.072212	43.609101
3518.531548	591764.616501	43.614106
3518.450040	591370.417396	43.619111
3518.604385	590965.163739	43.624116
3518.195043	590575.213739	43.629121
3518.282613	590172.707323	43.634125
3518.093235	589778.122009	43.639130
3518.132304	589389.915346	43.644135
3518.342731	589002.370154	43.649140
3518.124901	588604.133366	43.654145
3518.033703	588208.926624	43.659149
3517.981737	587820.985906	43.664154
3517.979503	587427.999270	43.669159
3518.258895	587043.544429	43.674164
3517.816820	586649.250603	43.679169
3518.117096	586260.294702	43.684173
3517.757038	585882.344293	43.689178
3517.869465	585495.154655	43.694183
3518.029298	585101.209889	43.699188
3517.644013	584723.880814	43.704193
3517.793689	584334.536673	43.709197
3517.841006	583962.286895	43.714202
3517.577198	583581.081450	43.719207
3517.853775	583181.273820	43.724212
3517.414265	582817.114597	43.729217
3517.711866	582428.287225	43.734221
3517.808915	582052.954272	43.739226
3517.499095	581675.416970	43.744231
3517.711747	581290.388511	43.749236
3517.184578	580917.791741	43.754241
3517.301648	580539.593427	43.759245
3517.924276	580170.045601	43.764250
3516.989841	579789.640580	43.769255
3517.528304	579416.162575	43.774260
3517.592279	579051.050966	43.779265
3517.534425	578670.411361	43.784269
3517.194978	578296.244719	43.789274
3517.003902	577913.090170	43.794279
3517.389871	577546.672144	43.799284
3517.254435	577187.121543	43.804289
3517.355246	576813.287463	43.809293
3517.516632	576443.807332	43.814298
3517.501538	576073.591910	43.819303
3517.179613	575690.541870	43.824308
3517.096016	575331.582540	43.829313
3517.158728	574954.982977	43.834317
3516.653087	574586.416689	43.839322
3516.408401	574229.565808	43.844327
3516.640550	573867.643222	43.849332
3516.592636	573507.267163	43.854337
3516.890129	573149.991117	43.859341
3516.875285	572794.116560	43.864346
3516.837071	572424.601929	43.869351
3516.646104	572069.743143	43.874356
3516.382010	571722.031257	43.879361
3516.764675	571359.960451	43.884365
3516.515770	571008.201169	43.889370
3516.357655	570652.290603	43.894375
3516.687327	570294.324328	43.899380
3516.420563	569939.217370	43.904385
3516.418862	569591.553080	43.909389
3516.576287	569234.290812	43.914394
3516.200817	568874.844911	43.919399
3516.144167	568524.443336	43.924404
3516.218927	568189.107731	43.929409
3516.447038	567830.032587	43.934413
3516.463737	567489.152420	43.939418
3516.384831	567143.045085	43.944423
3516.774253	566781.195103	43.949428
3516.243947	566433.031707	43.954433
3516.275451	566081.491170	43.959437
3516.060881	565738.540222	43.964442
3515.841724	565385.865734	43.969447
3516.122573	565046.939479	43.974452
3515.965633	564701.685836	43.979457
3515.942579	564356.953864	43.984461
3515.789450	564019.987749	43.989466
3515.787030	563673.421693	43.994471
3516.017256	563333.049526	43.999476
3515.722971	563010.832571	44.004481
3515.576417	562658.675507	44.009485
3515.595431	562324.757577	44.014490
3515.576908	561999.648908	44.019495
3515.712353	561652.804041	44.024500
3515.600227	561322.709610	44.029505
3515.588249	560992.589741	44.034509
3515.688938	560661.133049	44.039514
3515.703896	560334.667983	44.044519
3515.693489	559990.724682	44.049524
3515.526780	559673.036571	44.054529
3515.537448	559335.417855	44.059533
3515.701867	559001.893946	44.064538
3515.856564	558668.715800	44.069543
3516.142657	558329.362277	44.074548
3515.978459	557998.387352	44.079553
3515.883637	557659.736428	44.084557
3515.798414	557322.888479	44.089562
3515.614087	556985.797036	44.094567
3515.772988	556647.882855	44.099572
3515.568098	556316.117283	44.104577
3515.277170	555982.947653	44.109581
3515.280092	555653.145023	44.114586
3515.018152	555330.986290	44.119591
3515.327962	555004.742330	44.124596
3514.947147	554685.812490	44.129601
3515.019707	554350.877543	44.134605
3515.039795	554032.014812	44.139610
3514.538139	553729.104045	44.144615
3514.872162	553403.119225	44.149620
3514.927362	553083.371439	44.154625
3514.878302	552771.191755	44.159629
3514.874090	552456.780141	44.164634
3514.765698	552138.700631	44.169639
3514.761236	551820.091984	44.174644
3514.583251	551510.676561	44.179649
3514.900437	551202.026177	44.184653
3514.968070	550886.003595	44.189658
3514.841297	550577.465179	44.194663
3514.924851	550255.629861	44.199668
3514.855891	549936.332788	44.204673
3515.034634	549623.940814	44.209677
3515.145081	549313.670087	44.214682
3514.513872	548993.892523	44.219687
3515.112003	548672.839144	44.224692
3514.457042	548371.397086	44.229697
3514.572677	548057.518367	44.234701
3514.815789	547748.953580	44.239706
3514.587044	547434.716156	44.244711
3514.686784	547125.304923	44.249716
3514.360624	546807.289253	44.254721
3514.296179	546504.697175	44.259725
3514.257271	546202.648600	44.264730
3514.019486	545901.786825	44.269735
3514.561691	545596.147368	44.274740
3514.106979	545303.224350	44.279745
3514.136565	544992.214398	44.284749
3514.414019	544694.716995	44.289754
3514.323574	544393.595592	44.294759
3514.260345	544090.799214	44.299764
3514.039966	543795.938862	44.304769
3514.150422	543494.158632	44.309773
3513.905382	543210.180824	44.314778
3513.680314	542908.041812	44.319783
3514.030080	542608.218433	44.324788
3513.760466	542325.184849	44.329793
3513.907225	542018.424914	44.334797
3513.863106	541736.046867	44.339802
3513.406708	541457.465156	44.344807
3513.836631	541163.698880	44.349812
3513.654657	540871.140387	44.354817
3513.148601	540593.911616	44.359821
3513.492116	540298.326511	44.364826
3513.389358	540013.906594	44.369831
3513.715746	539729.558971	44.374836
3513.627577	539451.479869	44.379841
3513.335564	539160.871610	44.384845
3513.482990	538877.949609	44.389850
3513.472564	538595.855912	44.394855
3513.764138	538313.906793	44.399860
3513.315481	538024.260299	44.404865
3513.184627	537744.490468	44.409869
3513.634747	537461.639874	44.414874
3513.445509	537194.479631	44.419879
3513.488464	536909.972551	44.424884
3513.375659	536635.877999	44.429889
3512.926485	536352.906734	44.434893
3513.392021	536081.679101	44.439898
3513.351554	535808.161686	44.444903
3513.246073	535522.643385	44.449908
3513.357662	535245.961466	44.454913
3513.407892	534972.664876	44.459917
3513.166952	534693.610880	44.464922
3513.073576	534423.103195	44.469927
3513.203181	534134.490023	44.474932
3512.836051	533875.320366	44.479937
3512.869308	533606.491182	44.484941
3512.808730	533328.792711	44.489946
3512.858123	533071.152106	44.494951
3512.946788	532801.087514	44.499956
3512.866283	532539.523894	44.504961
3512.837680	532274.515417	44.509965
3512.676251	532008.061414	44.514970
3512.707517	531741.922857	44.519975
3513.190925	531467.476804	44.524980
3513.122563	531209.419560	44.529985
3512.631945	530930.739361	44.534989
3512.654385	530661.302368	44.539994
3512.607750	530409.232659	44.544999
3512.432733	530143.100141	44.550004
3512.077363	529890.973278	44.555009
3512.587724	529627.338711	44.560013
3512.656591	529366.348759	44.565018
3512.339232	529112.536507	44.570023
3512.539808	528837.029507	44.575028
3512.794505	528590.025201	44.580033
3512.759830	528330.952506	44.585037
3512.639690	528077.139192	44.590042
3512.519394	527820.293017	44.595047
3512.872861	527556.042434	44.600052
3512.727768	527300.806699	44.605057
3512.854825	527034.364460	44.610061
3512.664383	526766.760143	44.615066
3512.299153	526511.598870	44.620071
3512.619853	526246.320919	44.625076
3512.620358	525997.045076	44.630081
3512.629086	525739.232126	44.635085
3512.338147	525480.052342	44.640090
3511.978875	525232.541552	44.645095
3512.433761	524975.144044	44.650100
3511.872302	524731.900207	44.655105
3511.820031	524478.569112	44.660109
3511.966589	524233.580704	44.665114
3511.527948	523995.504127	44.670119
3512.012239	523740.301837	44.675124
3511.973726	523499.473139	44.680129
3512.133204	523256.486160	44.685133
3512.190013	523015.078022	44.690138
3512.076199	522759.860216	44.695143
3512.161239	522509.350502	44.700148
3511.766137	522267.098651	44.705153
3511.764983	522016.090517	44.710157
3511.560644	521775.111065	44.715162
3511.575958	521538.382473	44.720167
3511.718363	521300.669029	44.725172
3511.519293	521066.747018	44.730177
3511.695732	520828.464876	44.735181
3511.731832	520594.242928	44.740186
3511.740385	520351.739994	44.745191
3511.505501	520106.699188	44.750196
3511.551096	519881.302360	44.755201
3511.475284	519638.145928	44.760205
3511.871036	519410.510728	44.765210
3511.627005	519176.062269	44.770215
3511.362486	518938.330872	44.775220
3511.494129	518706.134297	44.780225
3511.380062	518471.248788	44.785229
3511.856959	518238.683134	44.790234
3511.548762	518006.652067	44.795239
3511.021175	517768.997937	44.800244
3510.967385	517548.382047	44.805249
3510.910806	517322.510376	44.810253
3511.297957	517097.115250	44.815258
3511.004163	516877.591455	44.820263
3511.277819	516644.026140	44.825268
3510.821668	516420.735104	44.830273
3510.812967	516196.859298	44.835277
3511.029354	515978.144852	44.840282
3510.765517	515764.560869	44.845287
3511.083718	515531.173193	44.850292
3510.949190	515324.027148	44.855297
3510.674540	515098.059143	44.860301
3510.945646	514879.471401	44.865306
3510.430506	514668.087514	44.870311
3510.782190	514448.368531	44.875316
3510.750301	514231.187447	44.880321
3510.535146	514024.593572	44.885325
3510.794568	513814.227828	44.890330
3510.611360	513600.095103	44.895335
3511.009564	513380.504698	44.900340
3510.970753	513166.290850	44.905345
3510.478550	512945.330641	44.910349
3510.197977	512732.920504	44.915354
3510.148525	512526.985892	44.920359
3510.297478	512316.618872	44.925364
3510.445920	512110.948172	44.930369
3510.254661	511902.806376	44.935373
3510.445812	511698.133545	44.940378
3510.351637	511502.753650	44.945383
3510.339956	511286.993636	44.950388
3510.455117	511084.347007	44.955393
3510.617210	510874.665899	44.960397
3510.737925	510670.143343	44.965402
3510.543988	510467.693172	44.970407
3510.791406	510251.975842	44.975412
3510.468716	510050.098178	44.980417
3510.649235	509832.112520	44.985421
3510.677873	509626.530973	44.990426
3510.478258	509422.552352	44.995431
3510.662379	509211.531527	45.000436
3510.589725	508999.237772	45.005441
3510.284935	508788.547499	45.010445
3509.987474	508586.697459	45.015450
3510.062266	508391.604111	45.020455
3510.209380	508196.445488	45.025460
3510.062703	508000.525993	45.030465
3510.266708	507788.472121	45.035469
3510.177594	507588.696617	45.040474
3509.945356	507398.192326	45.045479
3510.207390	507192.691170	45.050484
3509.829757	507000.842315	45.055489
3509.773343	506808.077066	45.060493
3509.824051	506607.305114	45.065498
3509.896696	506419.062204	45.070503
3509.820272	506225.231923	45.075508
3509.767941	506034.781826	45.080513
3509.641298	505844.797090	45.085517
3509.841488	505652.580750	45.090522
3509.492175	505469.150290	45.095527
3509.888553	505274.216875	45.100532
3509.824240	505090.480707	45.105537
3509.790374	504900.165715	45.110541
3509.479598	504720.460897	45.115546
3509.638640	504525.862295	45.120551
3509.696666	504341.136255	45.125556
3509.461568	504155.952634	45.130561
3509.447847	503969.768591	45.135565
3509.655580	503774.293259	45.140570
3509.272023	503606.468666	45.145575
3509.857489	503410.418925	45.150580
3509.724930	503238.553841	45.155585
3509.693647	503049.885053	45.160589
3509.590023	502863.602595	45.165594
3509.119073	502684.357621	45.170599
3509.405928	502492.240735	45.175604
3508.947047	502323.151846	45.180609
3508.953049	502149.583215	45.185613
3509.353142	501976.147693	45.190618
3509.200133	501803.563173	45.195623
3509.372430	501612.416162	45.200628
3509.191419	501440.742693	45.205633
3508.921000	501272.470318	45.210637
3508.879416	501086.662665	45.215642
3508.976439	500930.458953	45.220647
3508.963787	500744.945876	45.225652
3508.409112	500586.979339	45.230657
3508.899806	500418.467147	45.235661
3509.143099	500242.663597	45.240666
3508.883167	500073.214185	45.245671
3508.858003	499907.313115	45.250676
3508.712218	499742.745698	45.255681
3508.870980	499590.412355	45.260685
3508.591921	499419.543639	45.265690
3508.607491	499258.938669	45.270695
3508.523548	499091.876403	45.275700
3508.687011	498925.882724	45.280705
3508.461051	498774.264961	45.285709
3508.667311	498606.844848	45.290714
3508.432576	498454.467119	45.295719
3508.586847	498288.670923	45.300724
3508.536747	498127.863944	45.305729
3508.560763	497965.576180	45.310733
3508.789420	497797.891248	45.315738
3508.532676	497642.576661	45.320743
3508.735361	497483.186908	45.325748
3508.489526	497327.361793	45.330753
3508.451496	497167.554967	45.335757
3508.912741	497005.082065	45.340762
3508.406157	496853.697041	45.345767
3508.311055	496688.180404	45.350772
3508.546883	496535.451929	45.355777
3508.556098	496379.574441	45.360781
3508.673249	496214.775536	45.365786
3508.478306	496069.450026	45.370791
3508.640309	495904.033486	45.375796
3508.707645	495750.315083	45.380801
3508.489145	495589.360730	45.385805
3508.626656	495427.383046	45.390810
3508.407212	495275.378388	45.395815
3508.339664	495121.070314	45.400820
3508.662990	494972.409707	45.405825
3508.513094	494824.536726	45.410829
3508.474752	494663.896845	45.415834
3508.321283	494509.344943	45.420839
3508.668051	494346.410681	45.425844
3508.454766	494187.364204	45.430849
3508.092741	494039.571161	45.435853
3508.215716	493883.600592	45.440858
3508.138554	493745.822548	45.445863
3508.429759	493591.236929	45.450868
3508.144608	493437.456505	45.455873
3508.185715	493288.829311	45.460877
3508.253964	493143.534869	45.465882
3508.286706	492995.159468	45.470887
3508.356464	492833.522651	45.475892
3508.357003	492695.368719	45.480897
3508.226894	492542.363133	45.485901
3508.599987	492390.534965	45.490906
3508.049847	492245.338451	45.495911
3508.180128	492087.124267	45.500916
3508.004835	491945.048321	45.505921
3507.884474	491800.482899	45.510925
3508.130085	491652.868927	45.515930
3508.199481	491509.432230	45.520935
3507.821455	491358.431426	45.525940
3507.882301	491232.852636	45.530945
3507.852642	491086.191438	45.535949
3508.155491	490945.340959	45.540954
3507.960264	490813.529338	45.545959
3507.991030	490660.631246	45.550964
3508.049395	490512.988850	45.555969
3508.199229	490373.525852	45.560973
3507.784931	490230.414036	45.565978
3507.769589	490099.325150	45.570983
3507.970047	489951.805469	45.575988
3507.907477	489814.802804	45.580993
3507.811105	489672.138030	45.585997
3508.147933	489523.933658	45.591002
3507.771201	489393.204696	45.596007
3507.899660	489250.498054	45.601012
3507.511506	489112.887647	45.606017
3507.772890	488979.617902	45.611021
3508.034690	488833.950354	45.616026
3507.788813	488700.107287	45.621031
3507.846152	488562.517643	45.626036
3507.814127	488434.151368	45.631041
3507.791439	488295.561274	45.636045
3507.581577	488150.626332	45.641050
3507.800719	488018.925052	45.646055
3507.773034	487868.947138	45.651060
3507.719284	487745.386644	45.656065
3507.374617	487609.882183	45.661069
3507.556609	487475.956637	45.666074
3507.309152	487361.180771	45.671079
3507.647795	487218.067334	45.676084
3507.579248	487093.391470	45.681089
3507.353886	486953.965046	45.686093
3507.685215	486821.931951	45.691098
3507.857336	486696.098859	45.696103
3507.380626	486569.110512	45.701108
3507.376945	486436.372629	45.706113
3507.428005	486310.911681	45.711117
3507.586334	486173.285954	45.716122
3507.157746	486045.627711	45.721127
3508.001099	485914.461890	45.726132
3507.553035	485792.776793	45.731137
3507.402547	485650.391971	45.736141
3507.581267	485519.134252	45.741146
3507.338025	485395.032833	45.746151
3507.400216	485268.398540	45.751156
3507.379215	485139.348284	45.756161
3507.354421	485020.622146	45.761165
3507.445813	484896.814350	45.766170
3507.314415	484770.614419	45.771175
3507.452350	484629.892864	45.776180
3507.289093	484510.124103	45.781185
3507.059030	484391.226336	45.786189
3507.345426	484262.876365	45.791194
3507.267247	484147.240806	45.796199
3507.335692	484022.570396	45.801204
3507.150959	483899.713795	45.806209
3506.854230	483784.416862	45.811213
3507.103689	483650.906199	45.816218
3507.140946	483538.840539	45.821223
3507.114811	483421.166795	45.826228
3507.192998	483293.503347	45.831233
3506.746601	483174.533128	45.836237
3507.214137	483054.798677	45.841242
3506.956072	482942.374758	45.846247
3507.203778	482827.535430	45.851252
3507.158126	482706.418394	45.856257
3506.778592	482589.761205	45.861261
3507.102028	482475.564698	45.866266
3506.735428	482357.942059	45.871271
3507.243878	482242.244563	45.876276
3506.789121	482123.521840	45.881281
3506.950587	482013.500720	45.886285
3507.081816	481887.842888	45.891290
3507.037829	481778.260352	45.896295
3506.823597	481663.492413	45.901300
3507.075628	481558.768073	45.906305
3506.846032	481431.650057	45.911309
3507.475555	481320.785463	45.916314
3506.930108	481211.993770	45.921319
3507.074550	481086.581168	45.926324
3507.206296	480968.965552	45.931329
3506.824563	480844.856016	45.936333
3506.916653	480728.814873	45.941338
3507.239859	480615.618996	45.946343
3507.010275	480494.366537	45.951348
3507.160509	480388.944042	45.956353
3506.368163	480275.075907	45.961357
3506.776886	480159.787007	45.966362
3506.731951	480059.812641	45.971367
3506.583240	479944.161927	45.976372
3507.047355	479823.394000	45.981377
3506.726644	479716.984874	45.986381
3506.713834	479611.484426	45.991386
3506.576435	479497.651428	45.996391
3506.446880	479393.182150	46.001396
3506.419923	479289.504768	46.006401
3506.258856	479187.672241	46.011405
3506.670531	479080.982442	46.016410
3506.663394	478988.134057	46.021415
3506.735570	478880.691016	46.026420
3506.847862	478769.342169	46.031425
3506.480116	478664.251200	46.036429
3506.644519	478550.107579	46.041434
3506.428509	478439.673445	46.046439
3506.767993	478332.535919	46.051444
3506.575687	478228.678193	46.056449
3506.399413	478128.968743	46.061453
3506.822037	478016.802859	46.066458
3506.712171	477916.169571	46.071463
3506.463328	477818.546637	46.076468
3506.670369	477708.440874	46.081473
3506.538618	477603.050326	46.086477
3506.782931	477497.594958	46.091482
3506.151150	477401.300952	46.096487
3506.357415	477290.737120	46.101492
3506.726632	477193.460997	46.106497
3506.269572	477091.971070	46.111501
3506.669570	476992.511438	46.116506
3506.438826	476882.829876	46.121511
3506.430152	476786.426237	46.126516
3506.402212	476685.873448	46.131521
3506.044333	476588.718261	46.136525
3506.646361	476482.233926	46.141530
3506.570743	476388.219417	46.146535
3506.296827	476280.212546	46.151540
3506.219388	476185.690965	46.156545
3506.076598	476082.318934	46.161549
3506.401217	475982.664159	46.166554
3506.165667	475894.649391	46.171559
3505.909237	475803.295806	46.176564
3506.246082	475705.055242	46.181569
3506.057933	475617.132325	46.186573
3506.430296	475515.086962	46.191578
3506.521072	475422.608837	46.196583
3506.033683	475328.507307	46.201588
3506.200222	475225.178920	46.206593
3506.269652	475140.855639	46.211597
3506.331464	475042.253404	46.216602
3506.105857	474940.155049	46.221607
3506.273963	474846.546796	46.226612
3506.280980	474757.421773	46.231617
3505.993143	474654.167775	46.236621
3505.831824	474564.817373	46.241626
3506.105797	474479.139531	46.246631
3506.056801	474383.034031	46.251636
3506.043730	474291.985891	46.256641
3506.252570	474208.242234	46.261645
3506.473721	474096.694516	46.266650
3506.156787	474012.685266	46.271655
3506.156079	473914.999235	46.276660
3506.421995	473831.396055	46.281665
3506.146159	473739.377245	46.286669
3506.483122	473634.744851	46.291674
3506.347321	473547.917277	46.296679
3506.127257	473443.632127	46.301684
3506.397866	473346.707059	46.306689
3505.945002	473250.310158	46.311693
3505.846765	473162.461516	46.316698
3506.016046	473081.454260	46.321703
3505.706954	472989.488061	46.326708
3505.993952	472901.724344	46.331713
3506.038058	472814.913277	46.336717
3505.743441	472718.993046	46.341722
3505.849346	472647.718410	46.346727
3505.779733	472554.088555	46.351732
3506.186213	472465.390783	46.356737
3505.775086	472374.401228	46.361741
3506.266181	472284.320732	46.366746
3505.820497	472201.236910	46.371751
3505.729586	472108.823956	46.376756
3505.354474	472018.181039	46.381761
3505.807769	471937.322914	46.386765
3505.828315	471853.195661	46.391770
3505.217629	471778.241577	46.396775
3505.334831	471701.288973	46.401780
3505.856744	471625.634425	46.406785
3505.620318	471551.375238	46.411789
3505.642710	471463.143485	46.416794
3505.408205	471382.704296	46.421799
3505.646722	471299.752892	46.426804
3505.846200	471224.962154	46.431809
3505.274529	471144.174328	46.436813
3505.508401	471053.878606	46.441818
3505.641657	470993.786371	46.446823
3505.499287	470904.820397	46.451828
3505.449403	470834.578454	46.456833
3505.270795	470758.027043	46.461837
3505.689353	470674.231751	46.466842
3505.462013	470602.550401	46.471847
3505.502218	470513.804657	46.476852
3505.341811	470452.494584	46.481857
3505.588598	470372.374102	46.486861
3505.937310	470283.929155	46.491866
3505.474668	470212.489103	46.496871
3505.371949	470137.644350	46.501876
3505.671366	470067.339909	46.506881
3505.250008	469994.473745	46.511885
3505.594161	469911.954066	46.516890
3505.633529	469846.049256	46.521895
3505.437978	469762.810647	46.526900
3505.717395	469679.338617	46.531905
3505.496082	469618.137542	46.536909
3505.385623	469530.831181	46.541914
3505.006777	469473.962023	46.546919
3505.233979	469391.156128	46.551924
3505.489766	469310.472431	46.556929
3505.301184	469248.707388	46.561933
3505.344245	469174.593740	46.566938
3504.990507	469107.791064	46.571943
3505.061958	469038.382850	46.576948
3505.289086	468964.186298	46.581953
3505.430430	468896.741150	46.586957
3505.391779	468828.110784	46.591962
3505.168459	468756.877651	46.596967
3505.376309	468691.953163	46.601972
3505.429769	468615.809361	46.606977
3505.318894	468550.381604	46.611981
3505.433358	468468.097493	46.616986
3505.509389	468402.536004	46.621991
3505.698787	468316.540572	46.626996
3505.690108	468244.661001	46.632001
3505.503752	468166.124853	46.637005
3505.530885	468094.897137	46.642010
3505.190957	468025.150220	46.647015
3505.448435	467948.766292	46.652020
3505.569071	467877.724429	46.657025
3505.243905	467806.201190	46.662029
3505.144719	467729.927945	46.667034
3505.203900	467655.248403	46.672039
3505.241107	467587.715093	46.677044
3505.443900	467522.280912	46.682049
3505.150533	467461.085204	46.687053
3505.674903	467386.274526	46.692058
3505.588973	467317.697461	46.697063
3505.241231	467237.563977	46.702068
3505.215679	467165.429936	46.707073
3504.907308	467108.339046	46.712077
3505.307263	467035.726590	46.717082
3505.355837	466965.352219	46.722087
3505.293784	466898.188045	46.727092
3505.462702	466833.415876	46.732097
3505.298098	466767.028652	46.737101
3505.601485	466690.378571	46.742106
3505.249150	466627.011876	46.747111
3505.309389	466550.402754	46.752116
3505.535539	466483.897172	46.757121
3505.571610	466415.144069	46.762125
3505.424095	466332.996840	46.767130
3505.576900	466268.124196	46.772135
3505.228630	466201.867704	46.777140
3505.379794	466136.538943	46.782145
3504.870456	466067.877726	46.787149
3505.276771	465991.511262	46.792154
3505.250904	465916.586172	46.797159
3505.221643	465860.203853	46.802164
3505.383940	465788.792513	46.807169
3505.098978	465720.750363	46.812173
3505.478746	465656.495527	46.817178
3505.319280	465595.726983	46.822183
3505.224701	465518.684228	46.827188
3505.267215	465452.915735	46.832193
3505.145170	465382.514052	46.837197
3505.310115	465312.975061	46.842202
3505.176790	465255.088827	46.847207
3505.081507	465186.303111	46.852212
3505.086657	465115.372095	46.857217
3504.985915	465063.356799	46.862221
3505.034267	464988.415439	46.867226
3505.100326	464934.040735	46.872231
3505.205459	464877.987260	46.877236
3505.422081	464805.651046	46.882241
3505.040933	464744.107036	46.887245
3505.415014	464672.452756	46.892250
3505.030378	464611.618239	46.897255
3504.764664	464551.675212	46.902260
3505.019892	464481.965828	46.907265
3504.877528	464420.126688	46.912269
3505.364987	464359.395804	46.917274
3504.874308	464297.767747	46.922279
3504.761017	464233.389719	46.927284
3505.370426	464175.170776	46.932289
3504.839171	464120.439782	46.937293
3504.930045	464048.730227	46.942298
3504.985461	463982.042536	46.947303
3504.667381	463930.517322	46.952308
3505.064638	463867.216262	46.957313
3504.820084	463807.571334	46.962317
3504.667647	463742.691689	46.967322
3504.670792	463688.526917	46.972327
3504.731579	463630.045345	46.977332
3505.100087	463584.482180	46.982337
3504.618009	463529.437116	46.987341
3504.903781	463471.626015	46.992346
3504.835787	463412.811101	46.997351
3504.788336	463357.843348	47.002356
3505.114510	463295.363277	47.007361
3504.597217	463250.203926	47.012365
3504.796225	463189.518655	47.017370
3504.684515	463138.108118	47.022375
3505.030693	463074.407856	47.027380
3505.072532	463015.218303	47.032385
3504.762610	462962.118371	47.037389
3504.826743	462898.567034	47.042394
3504.666725	462846.809289	47.047399
3504.552184	462794.131573	47.052404
3504.640121	462745.827486	47.057409
3504.613945	462684.773735	47.062413
3504.977117	462630.949927	47.067418
3504.933675	462577.752780	47.072423
3504.633340	462522.876533	47.077428
3504.756666	462466.711681	47.082433
3504.701004	462411.438645	47.087437
3504.895148	462357.794963	47.092442
3504.861300	462304.443423	47.097447
3504.933246	462241.800716	47.102452
3504.829211	462195.757618	47.107457
3504.742191	462145.505718	47.112461
3504.781067	462085.249750	47.117466
3504.703673	462028.256488	47.122471
3504.708733	461980.015341	47.127476
3505.119161	461918.327261	47.132481
3504.578749	461864.402274	47.137485
3504.605994	461803.792720	47.142490
3504.712077	461747.932798	47.147495
3504.459292	461709.261569	47.152500
3504.989792	461653.582279	47.157505
3505.064755	461595.193566	47.162509
3505.263054	461537.543727	47.167514
3505.116724	461473.871698	47.172519
3504.676914	461427.022678	47.177524
3504.930316	461355.174170	47.182529
3504.904430	461309.369026	47.187533
3504.943781	461244.144322	47.192538
3504.871994	461184.867312	47.197543
3504.845884	461130.903175	47.202548
3504.751713	461080.700455	47.207553
3504.611053	461021.840114	47.212557
3504.742941	460966.429649	47.217562
3504.776061	460912.606829	47.222567
3504.287969	460867.335658	47.227572
3505.026315	460817.699577	47.232577
3504.432752	460760.638759	47.237581
3504.658973	460720.819613	47.242586
3504.782880	460665.409669	47.247591
3504.544004	460604.031056	47.252596
3504.591570	460555.120380	47.257601
3504.199220	460506.639432	47.262605
3504.551576	460452.203411	47.267610
3504.600989	460405.724523	47.272615
3504.063953	460368.264764	47.277620
3504.608028	460318.812637	47.282625
3504.512645	460272.408837	47.287629
3504.677605	460221.146152	47.292634
3504.543976	460166.995038	47.297639
3505.101874	460121.442207	47.302644
3505.189984	460069.280059	47.307649
3504.564473	460016.175393	47.312653
3505.070788	459952.032287	47.317658
3505.035141	459900.752351	47.322663
3505.013495	459841.006657	47.327668
3505.088897	459784.893044	47.332673
3505.255057	459729.523951	47.337677
3504.958868	459663.793877	47.342682
3504.822025	459615.165766	47.347687
3504.759933	459559.176350	47.352692
3504.624481	459508.115158	47.357697
3503.982901	459469.556616	47.362701
3504.261265	459413.812734	47.367706
3504.605205	459376.048640	47.372711
3504.290840	459333.937096	47.377716
3504.781481	459287.329576	47.382721
3504.444846	459235.491165	47.387725
3504.839442	459183.730482	47.392730
3504.371244	459146.560742	47.397735
3504.275876	459088.041692	47.402740
3504.407506	459038.251372	47.407745
3504.196309	458997.692585	47.412749
3504.377583	458943.281652	47.417754
3504.376928	458897.162553	47.422759
3503.977352	458863.882964	47.427764
3504.188213	458826.089873	47.432769
3504.197871	458775.458154	47.437773
3504.377588	458746.285960	47.442778
3504.346249	458699.918240	47.447783
3504.380121	458661.952336	47.452788
3504.442243	458607.003341	47.457793
3504.238445	458566.999909	47.462797
3504.380472	458525.315543	47.467802
3504.291129	458476.625865	47.472807
3504.057629	458435.867019	47.477812
3504.263463	458391.637399	47.482817
3504.428643	458352.786898	47.487821
3504.238358	458302.441531	47.492826
3504.126642	458273.267728	47.497831
3503.997484	458225.091057	47.502836
3503.973640	458183.383620	47.507841
3504.228316	458154.704588	47.512845
3504.223870	458110.408888	47.517850
3504.450554	458077.730612	47.522855
3504.236454	458030.784358	47.527860
3504.194837	457995.414896	47.532865
3504.147693	457953.710960	47.537869
3504.009805	457902.747448	47.542874
3504.020223	457878.417782	47.547879
3504.091761	457838.619297	47.552884
3504.523750	457802.104282	47.557889
3504.015874	457752.825427	47.562893
3504.372331	457714.397182	47.567898
3504.166273	457672.263644	47.572903
3504.141463	457640.844005	47.577908
3504.298627	457599.104448	47.582913
3503.996819	457562.156770	47.587917
3504.196216	457520.815310	47.592922
3504.155825	457473.128517	47.597927
3503.919172	457445.647417	47.602932
3504.458675	457401.155907	47.607937
3504.078203	457361.484342	47.612941
3504.145793	457327.666273	47.617946
3504.395567	457281.247276	47.622951
3504.171938	457248.087012	47.627956
3504.425926	457201.819167	47.632961
3504.409545	457167.761743	47.637965
3504.343431	457123.423713	47.642970
3504.181822	457086.501908	47.647975
3504.371907	457048.810392	47.652980
3504.300018	456998.188115	47.657985
3504.073909	456966.497684	47.662989
3504.147719	456914.431129	47.667994
3504.556514	456882.986957	47.672999
3504.261273	456834.784628	47.678004
3504.463075	456799.929044	47.683009
3504.200775	456761.300520	47.688013
3504.357160	456722.701804	47.693018
3504.101473	456673.073128	47.698023
3504.341938	456648.601325	47.703028
3504.247793	456601.631255	47.708033
3504.290958	456570.502459	47.713037
3504.344034	456525.990706	47.718042
3504.543201	456484.343044	47.723047
3503.934803	456446.178504	47.728052
3504.013263	456403.081372	47.733057
3504.373931	456374.939268	47.738061
3504.813122	456329.144670	47.743066
3504.392031	456291.860222	47.748071
3504.316251	456246.153366	47.753076
3504.832795	456206.377053	47.758081
3504.043968	456156.584704	47.763085
3504.026782	456114.922537	47.768090
3504.209850	456073.479529	47.773095
3503.754054	456046.946318	47.778100
3503.888546	456012.100871	47.783105
3503.741993	455974.921025	47.788109
3504.057785	455934.367451	47.793114
3504.398966	455916.466996	47.798119
3504.385014	455868.923966	47.803124
3504.306483	455835.229727	47.808129
3504.270327	455793.874268	47.813133
3504.292719	455762.190206	47.818138
3504.102026	455718.022432	47.823143
3504.365150	455679.809012	47.828148
3504.090899	455635.756703	47.833153
3503.532491	455600.623352	47.838157
3503.973151	455568.614126	47.843162
3504.170998	455547.595112	47.848167
3503.794070	455510.403062	47.853172
3504.064828	455475.330671	47.858177
3503.694967	455448.021666	47.863181
3504.004727	455396.671261	47.868186
3504.158379	455369.728965	47.873191
3504.271952	455343.046924	47.878196
3504.190181	455297.592402	47.883201
3503.988692	455264.881312	47.888205
3504.031020	455219.658874	47.893210
3504.235943	455194.126904	47.898215
3504.354053	455163.185911	47.903220
3504.600210	455129.435062	47.908225
3504.456445	455083.128918	47.913229
3504.419633	455046.688985	47.918234
3504.438043	454999.138396	47.923239
3504.166584	454967.199128	47.928244
3504.152970	454912.607847	47.933249
3503.830786	454888.888972	47.938253
3503.710670	454861.333773	47.943258
3503.848943	454827.296701	47.948263
3503.570183	454795.307720	47.953268
3504.140666	454763.680591	47.958273
3503.852096	454738.384385	47.963277
3504.275970	454698.468878	47.968282
3504.188393	454668.677459	47.973287
3503.681424	454628.819372	47.978292
3504.212020	454583.106623	47.983297
3504.239332	454556.387591	47.988301
3503.884555	454526.489513	47.993306
3504.005446	454481.201332	47.998311
3503.841398	454463.994169	48.003316
3503.911319	454419.779079	48.008321
3504.156016	454392.160955	48.013325
3504.113275	454360.130992	48.018330
3503.623453	454325.997563	48.023335
3503.739981	454292.875769	48.028340
3504.330637	454265.654631	48.033345
3504.255051	454234.035615	48.038349
3504.269360	454199.562436	48.043354
3504.198147	454163.278877	48.048359
3504.050901	454122.902150	48.053364
3504.349486	454088.481629	48.058369
3503.766891	454058.621765	48.063373
3504.135663	454016.889406	48.068378
3504.142098	453996.307021	48.073383
3504.034180	453956.480871	48.078388
3504.157432	453919.707441	48.083393
3503.741826	453888.500799	48.088397
3503.918749	453863.884423	48.093402
3504.065374	453832.226844	48.098407
3504.265713	453785.859004	48.103412
3504.392715	453749.287401	48.108417
3504.411532	453722.365958	48.113421
3504.419059	453693.266586	48.118426
3504.362394	453645.725669	48.123431
3503.707423	453623.228099	48.128436
3503.795675	453589.805835	48.133441
3503.848547	453556.389558	48.138445
3504.234720	453519.012884	48.143450
3504.040367	453496.081668	48.148455
3504.028925	453457.809589	48.153460
3504.250466	453422.133755	48.158465
3504.057823	453395.957708	48.163469
3503.944666	453349.034079	48.168474
3503.959541	453323.836394	48.173479
3503.529722	453300.438220	48.178484
3503.846239	453251.920170	48.183489
3503.770727	453237.839923	48.188493
3503.741706	453225.221873	48.193498
3503.883704	453193.057153	48.198503
3503.878866	453148.700004	48.203508
3503.867857	453125.787763	48.208513
3503.857325	453106.728231	48.213517
3503.681593	453055.911107	48.218522
3504.051188	453033.846288	48.223527
3503.796809	453023.750654	48.228532
3504.154663	452978.621477	48.233537
3503.885847	452952.812738	48.238541
3503.684753	452933.886975	48.243546
3503.851295	452898.523796	48.248551
3503.657143	452856.986593	48.253556
3503.696433	452831.074397	48.258561
3503.538177	452823.395642	48.263565
3503.812013	452796.074572	48.268570
3503.753137	452759.076686	48.273575
3503.429459	452736.318791	48.278580
3504.237197	452702.113189	48.283585
3503.429368	452677.207275	48.288589
3503.416184	452642.229217	48.293594
3503.501330	452618.742337	48.298599
3503.495690	452603.382322	48.303604
3503.476322	452588.886475	48.308609
3503.667308	452578.258311	48.313613
3503.702737	452548.392113	48.318618
3504.013098	452515.082269	48.323623
3503.965444	452492.783938	48.328628
3504.354038	452462.198260	48.333633
3504.104368	452425.029566	48.338637
3504.071093	452401.207783	48.343642
3504.256131	452355.143515	48.348647
3503.991916	452335.112649	48.353652
3504.219618	452307.748115	48.358657
3504.197297	452277.789993	48.363661
3504.007700	452244.058110	48.368666
3504.123727	452205.812638	48.373671
3503.902707	452186.027738	48.378676
3504.109320	452145.840195	48.383681
3503.873426	452111.659725	48.388685
3503.971629	452076.560295	48.393690
3504.365933	452051.701849	48.398695
3503.852676	452016.149050	48.403700
3503.816931	451988.879774	48.408705
3503.632336	451975.679151	48.413709
3503.672478	451933.441014	48.418714
3504.083549	451892.001319	48.423719
3503.607722	451882.754104	48.428724
3503.894919	451855.125323	48.433729
3503.815716	451830.296764	48.438733
3503.721756	451802.986486	48.443738
3504.115733	451780.257092	48.448743
3503.989255	451748.288060	48.453748
3503.952033	451715.086978	48.458753
3503.577329	451698.065563	48.463757
3503.663523	451671.028540	48.468762
3503.733439	451634.665730	48.473767
3503.558644	451616.748239	48.478772
3503.568837	451592.106925	48.483777
3503.659529	451580.481402	48.488781
3503.885077	451549.516628	48.493786
3503.876768	451521.532270	48.498791
3503.745919	451497.168420	48.503796
3504.041671	451470.957236	48.508801
3503.740987	451437.547200	48.513805
3503.328414	451417.439379	48.518810
3503.598692	451394.527889	48.523815
3503.354618	451384.835285	48.528820
3503.348970	451359.030318	48.533825
3503.674052	451322.369896	48.538829
3503.874353	451295.667797	48.543834
3504.305939	451275.111503	48.548839
3503.648728	451253.727109	48.553844
3503.583779	451213.837626	48.558849
3503.382480	451199.473270	48.563853
3503.388777	451180.409089	48.568858
3503.889196	451160.145127	48.573863
3503.744245	451150.283389	48.578868
3503.585394	451102.652666	48.583873
3503.446190	451088.987429	48.588877
3503.388899	451062.988112	48.593882
3503.838538	451054.951402	48.598887
3503.497240	451037.974440	48.603892
3503.717289	450996.058577	48.608897
3503.600230	450977.927875	48.613901
3503.236657	450964.959968	48.618906
3503.407207	450946.729431	48.623911
3503.515083	450936.520220	48.628916
3503.446181	450915.694128	48.633921
3503.499671	450875.783774	48.638925
3503.353497	450846.858740	48.643930
3503.536293	450822.491244	48.648935
3503.310261	450818.473754	48.653940
3503.411269	450798.733945	48.658945
3503.601810	450790.741374	48.663949
3503.451335	450774.542824	48.668954
3503.776022	450731.290344	48.673959
3503.378331	450721.319455	48.678964
3503.517437	450696.148059	48.683969
3503.316114	450689.337778	48.688973
3503.626444	450667.838274	48.693978
3503.822015	450650.262317	48.698983
3503.276915	450627.337105	48.703988
3503.695136	450592.383330	48.708993
3503.520235	450578.875956	48.713997
3503.185509	450568.285829	48.719002
3503.771951	450552.011979	48.724007
3503.231553	450546.476376	48.729012
3503.581143	450525.629139	48.734017
3503.706513	450499.699333	48.739021
3503.217219	450480.465625	48.744026
3503.235256	450469.105395	48.749031
3503.035022	450457.376816	48.754036
3503.308275	450433.551137	48.759041
3503.562631	450423.975784	48.764045
3503.319711	450412.862886	48.769050
3503.696523	450400.123119	48.774055
3503.756465	450367.106100	48.779060
3503.868119	450330.581781	48.784065
3503.484168	450320.709756	48.789069
3503.748796	450299.166976	48.794074
3503.952910	450273.223443	48.799079
3503.522833	450246.627636	48.804084
3503.933547	450225.009133	48.809089
3503.588350	450208.387074	48.814093
3503.384185	450178.102059	48.819098
3503.664057	450148.494885	48.824103
3503.160269	450130.632288	48.829108
3503.575548	450120.725106	48.834113
3503.717956	450101.991614	48.839117
3503.264617	450092.993268	48.844122
3503.363682	450082.734443	48.849127
3503.379281	450061.994474	48.854132
3503.751852	450023.650484	48.859137
3503.581830	450004.057606	48.864141
3503.456822	449998.298821	48.869146
3503.460169	449975.532757	48.874151
3503.384527	449973.416122	48.879156
3503.517947	449950.323605	48.884161
3503.659531	449921.398857	48.889165
3503.527009	449893.687036	48.894170
3503.691586	449881.236706	48.899175
3503.568720	449878.114068	48.904180
3503.469087	449850.903603	48.909185
3503.332384	449820.048819	48.914189
3503.320456	449801.797738	48.919194
3503.630220	449777.559454	48.924199
3503.522150	449769.668185	48.929204
3503.549881	449758.001694	48.934209
3503.535007	449744.212940	48.939213
3503.710162	449724.560862	48.944218
3503.732394	449686.580294	48.949223
3503.309155	449675.447090	48.954228
3503.485871	449655.389054	48.959233
3503.844014	449642.499905	48.964237
3503.735444	449622.946881	48.969242
3503.913872	449587.221118	48.974247
3503.616409	449572.466431	48.979252
3503.966308	449549.843546	48.984257
3503.837855	449521.522094	48.989261
3503.407297	449495.331042	48.994266
3503.969650	449477.640770	48.999271
3503.597611	449468.678975	49.004276
3503.762001	449426.769470	49.009281
3503.600673	449407.732293	49.014285
3503.298017	449386.792477	49.019290
3503.739469	449370.238247	49.024295
3503.382722	449362.947030	49.029300
3503.575852	449339.590125	49.034305
3503.454113	449306.653160	49.039309
3503.223662	449288.743170	49.044314
3503.583425	449273.723940	49.049319
3503.595501	449266.166896	49.054324
3503.497075	449245.952632	49.059329
3503.440138	449240.334128	49.064333
3503.304748	449224.486730	49.069338
3503.388596	449192.832798	49.074343
3503.490080	449171.063193	49.079348
3503.352811	449152.832949	49.084353
3503.217166	449150.118020	49.089357
3503.161915	449145.868227	49.094362
3503.505961	449119.037396	49.099367
3503.373976	449117.640159	49.104372
3503.098745	449095.022115	49.109377
3503.356022	449097.361266	49.114381
3503.082909	449084.934494	49.119386
3503.575689	449065.126156	49.124391
3503.318941	449043.265473	49.129396
3503.468183	449015.808609	49.134401
3503.130524	448995.939183	49.139405
3503.187021	448982.847611	49.144410
3503.495090	448965.098918	49.149415
3503.097557	448975.155643	49.154420
3503.049977	448955.033827	49.159425
3503.313288	448937.444869	49.164429
3503.261805	448933.042273	49.169434
3503.461513	448923.576979	49.174439
3503.606633	448909.557537	49.179444
3503.580294	448880.457207	49.184449
3503.775485	448856.592362	49.189453
3503.406734	448841.342280	49.194458
3503.525162	448828.544269	49.199463
3503.093894	448817.158450	49.204468
3503.283046	448807.999139	49.209473
3503.157241	448793.316004	49.214477
3503.132453	448784.091801	49.219482
3503.224314	448783.112670	49.224487
3503.282561	448777.829313	49.229492
3503.399371	448736.433611	49.234497
3503.369143	448717.474834	49.239501
3503.430167	448699.159632	49.244506
3503.576743	448676.722643	49.249511
3503.755751	448683.588014	49.254516
3503.509782	448665.984376	49.259521
3503.491181	448645.096730	49.264525
3503.522645	448618.622870	49.269530
3503.678310	448609.215661	49.274535
3503.199514	448600.880193	49.279540
3503.032769	448586.457433	49.284545
3502.821560	448570.115428	49.289549
3502.849247	448560.476520	49.294554
3502.879310	448547.237073	49.299559
3502.859387	448543.386773	49.304564
3503.124517	448532.845306	49.309569
3503.350924	448523.780923	49.314573
3502.947845	448519.691806	49.319578
3503.261292	448510.460436	49.324583
3503.079886	448506.485585	49.329588
3503.133179	448481.579715	49.334593
3503.526017	448472.334774	49.339597
3503.381285	448468.353653	49.344602
3503.505181	448457.075670	49.349607
3503.243741	448452.455292	49.354612
3503.206682	448447.441657	49.359617
3503.365710	448439.149337	49.364621
3503.521904	448411.944031	49.369626
3503.448897	448380.670606	49.374631
3503.414944	448375.200065	49.379636
3503.347112	448353.407820	49.384641
3503.359433	448346.458882	49.389645
3503.487938	448336.042058	49.394650
3503.449186	448325.096016	49.399655
3503.289444	448304.637785	49.404660
3503.391791	448279.926128	49.409665
3503.247073	448258.603273	49.414669
3503.224705	448243.749973	49.419674
3503.492216	448228.948579	49.424679
3503.451739	448226.825763	49.429684
3503.268461	448213.267586	49.434689
3503.476321	448199.946856	49.439693
3503.433569	448201.272492	49.444698
3503.602660	448185.575150	49.449703
3503.216732	448152.884317	49.454708
3503.028186	448128.678516	49.459713
3503.262739	448122.959234	49.464717
3503.263924	448116.214950	49.469722
3503.174111	448105.176099	49.474727
3503.149181	448094.531820	49.479732
3503.245407	448078.441182	49.484737
3503.407239	448076.030271	49.489741
3503.293841	448068.697051	49.494746
3503.481151	448053.503571	49.499751
3503.251390	448045.987383	49.504756
3503.350168	448036.488218	49.509761
3503.028618	448029.799013	49.514765
3503.089215	448022.588189	49.519770
3502.992814	448008.457266	49.524775
3503.000387	448008.050272	49.529780
3503.127473	447992.917740	49.534785
3503.227688	447987.779141	49.539789
3503.095462	447988.055214	49.544794
3503.241741	447968.355722	49.549799
3503.334663	447946.484900	49.554804
3503.123593	447926.339311	49.559809
3503.421075	447914.169372	49.564813
3503.359210	447899.677526	49.569818
3503.161850	447887.845603	49.574823
3503.095884	447888.718854	49.579828
3503.400523	447878.778807	49.584833
3503.319250	447862.971852	49.589837
3502.955275	447869.575248	49.594842
3503.325005	447843.701858	49.599847
3503.214557	447848.892862	49.604852
3503.375658	447825.691874	49.609857
3503.324146	447823.621609	49.614861
3503.358246	447818.646382	49.619866
3503.886023	447793.202314	49.624871
3503.060964	447766.315849	49.629876
3503.487621	447745.047038	49.634881
3503.384117	447737.103517	49.639885
3503.549772	447727.592795	49.644890
3503.447186	447718.584243	49.649895
3503.263783	447712.733385	49.654900
3503.210514	447704.172777	49.659905
3502.947971	447710.048990	49.664909
3502.925489	447695.043200	49.669914
3503.465652	447683.186647	49.674919
3503.043477	447678.289295	49.679924
3503.203458	447647.634208	49.684929
3503.383503	447622.857809	49.689933
3503.096048	447602.420704	49.694938
3503.293171	447601.119296	49.699943
3503.174592	447591.504921	49.704948
3503.170561	447573.706935	49.709953
3502.834380	447575.133421	49.714957
3502.730716	447569.066075	49.719962
3502.930950	447548.342812	49.724967
3502.811554	447560.228927	49.729972
3502.829684	447577.162390	49.734977
3503.257722	447576.024385	49.739981
3502.968049	447578.558515	49.744986
3503.178030	447568.888028	49.749991
3503.020284	447559.787409	49.754996
3503.227557	447553.565549	49.760001
3503.576165	447550.869145	49.765005
3503.610267	447524.647006	49.770010
3503.624037	447490.010685	49.775015
3503.479607	447485.572950	49.780020
3503.274901	447475.719684	49.785025
3503.254085	447462.437537	49.790029
3503.232459	447457.573158	49.795034
3503.322121	447452.081271	49.800039
3503.274485	447448.387630	49.805044
3502.948128	447428.717630	49.810049
3502.898437	447409.507458	49.815053
3502.787510	447417.386214	49.820058
3502.933785	447398.345407	49.825063
3503.007856	447409.285814	49.830068
3503.061438	447395.382416	49.835073
3503.462766	447384.056492	49.840077
3503.193520	447380.806349	49.845082
3503.272964	447371.513023	49.850087
3503.008718	447373.434328	49.855092
3503.290924	447356.956425	49.860097
3503.480887	447354.084250	49.865101
3503.359668	447317.746594	49.870106
3503.267734	447294.233267	49.875111
3502.749972	447289.707108	49.880116
3502.863145	447281.929256	49.885121
3502.795471	447270.683352	49.890125
3502.777830	447286.254010	49.895130
3502.941138	447283.893466	49.900135
3502.980896	447290.935195	49.905140
3503.146514	447285.075332	49.910145
3502.932191	447279.990269	49.915149
3502.837633	447280.716300	49.920154
3503.176505	447259.107029	49.925159
3502.949075	447265.383041	49.930164
3502.929937	447257.729190	49.935169
3503.368311	447245.179847	49.940173
3503.151633	447236.799080	49.945178
3503.232007	447230.345248	49.950183
3502.944773	447218.071913	49.955188
3503.160806	447212.304840	49.960193
3503.094412	447206.636700	49.965197
3502.695166	447205.893480	49.970202
3502.989110	447185.356699	49.975207
3503.255405	447186.122537	49.980212
3503.243799	447184.704616	49.985217
3503.088954	447170.228148	49.990221
3503.210768	447172.235680	49.995226
3503.619059	447159.184329	50.000231
3503.694066	447148.116836	50.005236
3503.598058	447117.048307	50.010241
3503.533962	447101.035013	50.015245
3503.424770	447089.289007	50.020250
3503.899957	447081.753525	50.025255
3503.946238	447064.859294	50.030260
3503.518349	447046.068338	50.035265
3503.857303	447018.779329	50.040269
3503.554336	447012.695143	50.045274
3503.891729	446994.635536	50.050279
3503.805485	446968.382549	50.055284
3503.645038	446952.588434	50.060289
3503.600923	446936.368764	50.065293
3503.302281	446922.423778	50.070298
3503.528415	446893.835415	50.075303
3503.294333	446884.696830	50.080308
3503.526601	446866.097254	50.085313
3503.622898	446852.186207	50.090317
3503.509378	446854.842474	50.095322
3503.466873	446841.411511	50.100327
3503.677884	446822.663396	50.105332
3503.666942	446791.478446	50.110337
3503.751069	446772.802663	50.115341
3503.329259	446759.182862	50.120346
3503.126563	446749.227495	50.125351
3503.040236	446749.901428	50.130356
3503.513737	446738.055734	50.135361
3503.104262	446729.606265	50.140365
3503.168122	446723.662203	50.145370
3503.528679	446708.742443	50.150375
3503.324323	446686.921084	50.155380
3503.170066	446668.285912	50.160385
3503.322464	446652.387445	50.165389
3502.914865	446658.745110	50.170394
3503.197941	446638.006816	50.175399
3502.929440	446635.263536	50.180404
3502.894940	446626.699289	50.185409
3502.813341	446624.786176	50.190413
3502.799754	446627.678961	50.195418
3502.955787	446641.242721	50.200423
3502.874040	446645.110643	50.205428
3503.104649	446644.057013	50.210433
3503.283073	446636.115651	50.215437
3502.947706	446625.523641	50.220442
3502.967437	446614.211755	50.225447
3503.356739	446613.587423	50.230452
3503.065270	446599.235315	50.235457
3503.105187	446598.518508	50.240461
3502.921580	446596.572099	50.245466
3502.873723	446575.890250	50.250471
3502.974849	446585.710825	50.255476
3502.870125	446570.464729	50.260481
3503.065287	446566.577345	50.265485
3502.580773	446561.031136	50.270490
3502.940939	446553.565819	50.275495
3502.876386	446553.931775	50.280500
3502.715934	446551.220746	50.285505
3503.070045	446546.393423	50.290509
3502.986467	446539.308135	50.295514
3503.438918	446522.749808	50.300519
3502.952026	446517.863235	50.305524
3503.121721	446513.016682	50.310529
3503.147704	446502.362911	50.315533
3502.958991	446505.539169	50.320538
3502.923852	446495.656495	50.325543
3502.950944	446488.552293	50.330548
3503.375134	446477.881227	50.335553
3503.143844	446480.202672	50.340557
3502.899285	446475.173289	50.345562
3503.167926	446459.964784	50.350567
3502.784474	446460.131638	50.355572
3503.094821	446450.037819	50.360577
3503.095062	446443.090320	50.365581
3503.462810	446442.114686	50.370586
3503.123611	446431.117545	50.375591
3502.990832	446429.618842	50.380596
3503.105894	446422.246042	50.385601
3503.278925	446417.246765	50.390605
3503.243779	446411.623787	50.395610
3503.257141	446390.677750	50.400615
3503.182881	446393.986615	50.405620
3502.822951	446386.948463	50.410625
3503.212445	446369.690810	50.415629
3502.946705	446380.740481	50.420634
3503.182057	446377.404023	50.425639
3503.057783	446368.246467	50.430644
3502.927667	446362.386136	50.435649
3503.125774	446351.094364	50.440653
3503.120793	446352.058687	50.445658
3503.105114	446337.202910	50.450663
3503.166174	446339.423740	50.455668
3503.159210	446338.816351	50.460673
3503.474285	446326.135388	50.465677
3502.982257	446322.821699	50.470682
3503.154900	446312.852750	50.475687
3503.038918	446310.742634	50.480692
3503.003169	446303.091275	50.485697
3502.641071	446295.089946	50.490701
3502.573577	446296.318502	50.495706
3503.019369	446283.310926	50.500711
3502.910097	446283.126696	50.505716
3503.002348	446277.634065	50.510721
3502.993654	446271.803688	50.515725
3502.941763	446272.268910	50.520730
3502.795556	446259.413113	50.525735
3502.864812	446249.867480	50.530740
3502.862921	446214.775353	50.535745
3503.046926	446170.269761	50.540749
3502.744777	446113.270549	50.545754
3502.880689	446048.488163	50.550759
3503.011329	445970.774875	50.555764
3502.974421	445879.904692	50.560769
3502.963333	445771.483138	50.565773
3503.003750	445658.234512	50.570778
3502.984446	445526.637297	50.575783
3502.728215	445393.203327	50.580788
3502.826764	445241.552372	50.585793
3502.911578	445077.376261	50.590797
3502.639025	444916.708514	50.595802
3502.654900	444727.234854	50.600807
3502.847322	444541.533050	50.605812
3502.699483	444336.362071	50.610817
3503.065604	444109.394694	50.615821
3502.725785	443875.140769	50.620826
3502.858073	443627.921397	50.625831
3503.021865	443374.151161	50.630836
3503.129922	443110.700159	50.635841
3503.113069	442822.110381	50.640845
3502.687662	442524.710482	50.645850
3502.856113	442209.300604	50.650855
3502.826781	441890.267970	50.655860
3502.577223	441557.826814	50.660865
3502.798143	441204.097920	50.665869
3502.419594	440850.414959	50.670874
3502.725775	440463.587392	50.675879
3502.220954	440089.775902	50.680884
3502.398100	439695.500181	50.685889
3502.353103	439275.688571	50.690893
3502.106328	438866.810145	50.695898
3502.207781	438422.506133	50.700903
3502.574453	437968.864245	50.705908
3502.404245	437494.961355	50.710913
3502.233550	437020.490456	50.715917
3502.170173	436524.277047	50.720922
3502.259216	436014.784796	50.725927
3501.999449	435487.684360	50.730932
3501.807092	434941.787245	50.735937
3501.945148	434387.448689	50.740941
3501.868241	433818.926136	50.745946
3501.743693	433227.158033	50.750951
3501.897049	432628.071006	50.755956
3502.108981	432008.863741	50.760961
3501.858954	431367.340013	50.765965
3501.693174	430719.745272	50.770970
3502.006570	430036.679093	50.775975
3501.531790	429351.697542	50.780980
3501.404471	428641.260974	50.785985
3501.895767	427916.435779	50.790989
3501.321213	427184.918526	50.795994
3501.293725	426412.122118	50.800999
3501.064462	425636.543475	50.806004
3501.319367	424855.172026	50.811009
3500.968701	424041.645324	50.816013
3500.834906	423218.815421	50.821018
3501.152507	422363.695845	50.826023
3500.730126	421504.916030	50.831028
3500.702192	420614.511793	50.836033
3500.833820	419698.688579	50.841037
3500.610980	418792.818109	50.846042
3500.641191	417838.179471	50.851047
3500.599301	416888.213704	50.856052
3500.344405	415907.071113	50.861057
3500.430925	414909.608303	50.866061
3500.174314	413892.512735	50.871066
3500.262781	412847.336275	50.876071
3499.769614	411798.484330	50.881076
3499.591245	410724.294970	50.886081
3499.420047	409629.769964	50.891085
3499.151777	408528.740389	50.896090
3499.121734	407401.719703	50.901095
3499.257662	406267.664410	50.906100
3499.437762	405101.322495	50.911105
3499.281628	403917.334999	50.916109
3498.996590	402712.337051	50.921114
3498.576047	401491.433396	50.926119
3498.668944	400256.594695	50.931124
3498.427900	399005.550831	50.936129
3498.674887	397722.204839	50.941133
3498.112858	396435.992590	50.946138
3498.187506	395115.110314	50.951143
3498.318758	393786.891843	50.956148
3498.301536	392436.277923	50.961153
3498.002245	391061.789639	50.966157
3497.861629	389680.528208	50.971162
3498.033942	388261.690633	50.976167
3497.840669	386839.978408	50.981172
3497.032988	385399.320354	50.986177
3497.091194	383928.913546	50.991181
3496.305461	382458.303579	50.996186
3496.308169	380965.808926	51.001191
3496.517264	379468.736856	51.006196
3495.862315	377952.932251	51.011201
3495.893821	376407.679646	51.016205
3495.397826	374864.429949	51.021210
3495.240579	373283.346975	51.026215
3495.125601	371703.253064	51.031220
3494.685820	370115.388515	51.036225
3494.633358	368492.219132	51.041229
3494.861547	366864.987753	51.046234
3494.316619	365212.665118	51.051239
3494.130081	363565.269534	51.056244
3494.073707	361879.782727	51.061249
3493.742619	360185.799668	51.066253
3493.031302	358487.026650	51.071258
3493.099335	356763.374641	51.076263
3492.845324	355029.758369	51.081268
3492.439889	353295.255870	51.086273
3492.490751	351517.279697	51.091277
3492.175147	349736.544845	51.096282
3491.794191	347945.724494	51.101287
3491.287424	346142.335733	51.106292
3490.893542	344327.686274	51.111297
3491.007733	342474.075360	51.116301
3490.438570	340630.356415	51.121306
3490.503570	338768.646155	51.126311
3490.636400	336894.995680	51.131316
3490.389606	335007.191274	51.136321
3490.206482	333089.251145	51.141325
3489.547408	331176.693407	51.146330
3489.029672	329238.185721	51.151335
3489.174350	327299.930672	51.156340
3488.545675	325337.790901	51.161345
3488.848717	323357.583704	51.166349
3488.081984	321372.073073	51.171354
3487.950813	319369.004942	51.176359
3487.810626	317357.399538	51.181364
3487.464774	315335.331439	51.186369
3487.206784	313286.000170	51.191373
3486.923698	311236.818479	51.196378
3486.173846	309176.559880	51.201383
3486.061106	307105.495388	51.206388
3485.562655	305008.346274	51.211393
3485.429130	302902.502109	51.216397
3485.101319	300796.411600	51.221402
3484.489193	298666.437602	51.226407
3483.951915	296532.839154	51.231412
3483.363766	294397.626037	51.236417
3483.446231	292253.700142	51.241421
3482.457807	290092.982899	51.246426
3481.997035	287921.314489	51.251431
3481.985934	285746.426222	51.256436
3481.290876	283562.987950	51.261441
3481.017317	281363.809833	51.266445
3480.367697	279176.584848	51.271450
3480.403629	276954.683145	51.276455
3480.177191	274730.229332	51.281460
3479.609049	272505.531630	51.286465
3479.232636	270248.055920	51.291469
3478.578326	267997.206640	51.296474
3478.505804	265726.786228	51.301479
3477.771894	263450.940519	51.306484
3477.347942	261173.504935	51.311489
3477.183639	258879.897680	51.316493
3476.798399	256580.110800	51.321498
3476.026910	254271.195708	51.326503
3475.935888	251951.215963	51.331508
3474.921715	249632.876934	51.336513
3474.842010	247290.574776	51.341517
3474.612284	244957.122369	51.346522
3474.102841	242608.274201	51.351527
3473.625748	240243.751279	51.356532
3472.984858	237873.701180	51.361537
3472.813031	235490.837607	51.366541
3472.020923	233112.565686	51.371546
3471.312173	230724.940262	51.376551
3470.775190	228319.724540	51.381556
3470.152537	225921.566180	51.386561
3469.931970	223515.055081	51.391565
3468.865848	221112.631045	51.396570
3468.709039	218693.168192	51.401575
3468.249714	216266.783202	51.406580
3467.460864	213845.350207	51.411585
3467.201503	211407.643196	51.416589
3466.394440	208963.271572	51.421594
3466.096248	206519.480747	51.426599
3465.693326	204066.246090	51.431604
3464.941203	201608.947465	51.436609
3464.378121	199132.018547	51.441613
3463.705130	196666.891930	51.446618
3463.294921	194193.816083	51.451623
3462.773298	191725.027054	51.456628
3461.942435	189230.513239	51.461633
3461.151800	186744.634401	51.466637
3460.633522	184261.423285	51.471642
3459.926964	181771.646970	51.476647
3459.143245	179269.539540	51.481652
3458.486978	176777.758885	51.486657
3457.885679	174278.799333	51.491661
3456.995900	171788.322757	51.496666
3456.192220	169282.680623	51.501671
3456.065270	166784.969755	51.506676
3455.080269	164281.220155	51.511681
3454.886653	161771.625673	51.516685
3453.775016	159272.458680	51.521690
3452.918550	156764.417489	51.526695
3452.131136	154263.767333	51.531700
3451.519501	151770.708663	51.536705
3450.999443	149255.794810	51.541709
3449.757215	146742.569194	51.546714
3449.034532	144245.864592	51.551719
3448.720514	141713.320395	51.556724
3447.505139	139173.927973	51.561729
3447.107167	136671.064164	51.566733
3445.852072	134176.945388	51.571738
3445.526686	131683.642508	51.576743
3444.746856	129182.384973	51.581748
3443.609836	126691.651858	51.586753
3442.988310	124197.711880	51.591757
3441.772223	121715.586910	51.596762
3440.928524	119230.019507	51.601767
3439.829825	116752.592913	51.606772
3438.844331	114291.362948	51.611777
3438.506475	111811.702549	51.616781
3437.233694	109357.656055	51.621786
3436.273639	106893.601887	51.626791
3435.784080	104450.375832	51.631796
3434.625984	101999.284934	51.636801
3433.781687	99555.795739	51.641805
3432.449823	97128.888355	51.646810
3431.373079	94696.665842	51.651815
3430.372101	92293.940220	51.656820
3428.943328	89891.019749	51.661825
3428.220125	87496.977812	51.666829
3426.976276	85116.490916	51.671834
3426.017929	82742.709306	51.676839
3424.804458	80377.001568	51.681844
3423.551739	78027.747837	51.686849
3422.903972	75686.706421	51.691853
3421.475457	73371.913554	51.696858
3419.897022	71059.195303	51.701863
3418.931904	68757.001220	51.706868
3417.296877	66478.278682	51.711873
3415.991133	64203.844299	51.716877
3414.756224	61950.696680	51.721882
3413.743255	59715.339800	51.726887
3412.155673	57497.786396	51.731892
3410.963133	55308.182008	51.736897
3409.585198	53116.339126	51.741901
3408.078234	50963.125351	51.746906
3406.871861	48813.895928	51.751911
3405.710891	46688.906434	51.756916
3403.823978	44587.608740	51.761921
3402.452797	42485.663136	51.766925
3400.609570	40429.242183	51.771930
3399.085872	38399.635510	51.776935
3397.367082	36385.133035	51.781940
3395.294667	34403.469392	51.786945
3394.043990	32448.081989	51.791949
3392.304762	30534.234011	51.796954
3390.145926	28626.002495	51.801959
3388.351314	26761.638625	51.806964
3386.227228	24924.875947	51.811969
3384.203996	23121.964701	51.816973
3381.107938	21369.829240	51.821978
3377.541588	19712.297482	51.826983
3372.146760	18131.574475	51.831988
3366.071798	16642.684673	51.836993
3360.975682	15240.126473	51.841997
3354.680672	13951.956079	51.847002
3348.567626	12780.134920	51.852007
3342.143929	11727.162440	51.857012
3336.292069	10794.914615	51.862017
3330.914307	9958.888449	51.867021
3326.072369	9237.329304	51.872026
3322.076691	8603.586487	51.877031
3318.023138	8071.049204	51.882036
3314.544014	7628.871246	51.887041
3311.927412	7252.622426	51.892045
3309.442856	6961.005227	51.897050
3307.394318	6711.757027	51.902055
3305.724447	6508.610225	51.907060
3304.259495	6359.514110	51.912065
3303.342268	6244.870708	51.917069
3302.325649	6163.456716	51.922074
3301.739632	6109.403248	51.927079
3300.860381	6062.437531	51.932084
3300.366692	6046.513563	51.937089
3300.411160	6031.255839	51.942093
3299.835641	6030.749163	51.947098
3299.428096	6032.324795	51.952103
3299.597460	6057.681577	51.957108
3299.648365	6084.184033	51.962113
3299.459132	6095.685113	51.967117
3299.181442	6116.016549	51.972122
3298.992927	6135.884987	51.977127
3299.065900	6149.816407	51.982132
3298.887367	6173.470856	51.987137
3298.977355	6177.596930	51.992141
3299.227766	6196.220829	51.997146
3298.612348	6199.770845	52.002151
3298.820971	6191.398475	52.007156
3298.160799	6195.597418	52.012161
3298.400998	6186.982729	52.017165
3298.292148	6176.783396	52.022170
3298.083719	6160.969325	52.027175
3298.137674	6148.615384	52.032180
3297.884800	6110.484146	52.037185
3298.004643	6066.440424	52.042189
3297.588454	6030.585700	52.047194
3297.783206	5978.023815	52.052199
3297.585952	5927.998602	52.057204
3296.493134	5886.773428	52.062209
3296.050045	5823.542602	52.067213
3295.612277	5772.788964	52.072218
3295.136716	5712.791780	52.077223
3294.923302	5650.414802	52.082228
3294.093419	5609.552141	52.087233
3294.058287	5529.393650	52.092237
3293.149468	5473.815657	52.097242
3292.748903	5418.216581	52.102247
3292.713249	5348.957224	52.107252
3291.486367	5282.693300	52.112257
3291.192392	5208.721447	52.117261
3290.703988	5137.881169	52.122266
3290.262944	5069.618601	52.127271
3289.678337	4990.667002	52.132276
3288.804304	4934.254187	52.137281
3288.397435	4850.405234	52.142285
3287.857806	4781.231275	52.147290
3287.002484	4719.954702	52.152295
3286.928075	4654.974018	52.157300
3286.149884	4578.878276	52.162305
3285.267341	4496.589934	52.167309
3284.935099	4436.930791	52.172314
3284.180656	4356.163521	52.177319
3283.805154	4278.921738	52.182324
3282.860027	4213.562527	52.187329
3282.771006	4132.910139	52.192333
3281.777277	4057.742078	52.197338
3280.830710	3978.933142	52.202343
3280.394197	3912.971853	52.207348
3279.738787	3840.617387	52.212353
3279.319950	3759.939534	52.217357
3278.437643	3691.038118	52.222362
3278.008866	3624.449737	52.227367
3277.607962	3551.488527	52.232372
3276.246203	3471.329347	52.237377
3275.970671	3389.340234	52.242381
3275.556753	3329.259390	52.247386
3274.819818	3250.387474	52.252391
3274.301578	3170.387351	52.257396
3273.290239	3102.739961	52.262401
3272.949434	3030.665508	52.267405
3271.987145	2959.124725	52.272410
3271.288744	2887.738164	52.277415
3271.113142	2811.150014	52.282420
3270.264066	2744.768998	52.287425
3269.677854	2657.270954	52.292429
3268.860735	2592.356114	52.297434
3268.090367	2527.020606	52.302439
3267.660277	2448.443742	52.307444
3266.890778	2380.496788	52.312449
3266.392754	2309.345487	52.317453
3265.944669	2244.676177	52.322458
3264.889043	2176.401574	52.327463
3264.599963	2101.280357	52.332468
3263.770125	2043.284878	52.337473
3263.214184	1966.347341	52.342477
3262.549377	1896.594685	52.347482
3262.006048	1819.786775	52.352487
3261.320581	1746.139563	52.357492
3260.384086	1685.810804	52.362497
3259.885502	1604.128035	52.367501
3259.353295	1541.447049	52.372506
3258.361749	1471.646301	52.377511
3258.365797	1402.556887	52.382516
3257.232597	1335.845860	52.387521
3256.374255	1261.440939	52.392525
3255.537438	1196.802873	52.397530
3254.906258	1127.643574	52.402535
3254.278623	1064.852894	52.407540
3253.414042	1013.611094	52.412545
3252.698157	949.924474	52.417549
3251.975192	896.316033	52.422554
3251.364087	844.022117	52.427559
3250.859134	779.199999	52.432564
3249.860605	730.481138	52.437569
3249.343730	675.580199	52.442573
3248.476787	625.999174	52.447578
3247.893367	572.518795	52.452583
3247.341746	520.078037	52.457588
3246.240857	479.156154	52.462593
3245.417809	427.297736	52.467597
3244.621032	396.915265	52.472602
3243.562295	358.313855	52.477607
3242.989016	320.781830	52.482612
3241.518582	303.988049	52.487617
3241.180578	281.872072	52.492621
3240.160822	271.911508	52.497626
3239.341102	240.147363	52.502631
3238.576174	226.081122	52.507636
3237.638677	212.423711	52.512641
3236.996121	204.270956	52.517645
3236.520825	189.093050	52.522650
3235.389399	186.058204	52.527655
3235.292721	170.512876	52.532660
3234.692813	166.847240	52.537665
3233.459493	154.278951	52.542669
3232.884253	163.112923	52.547674
3231.981097	161.669710	52.552679
3231.504635	160.335569	52.557684
3231.002796	161.277034	52.562689
3230.158347	157.588048	52.567693
3229.406091	157.293373	52.572698
3228.991781	161.200479	52.577703
3228.453838	156.887168	52.582708
3227.451383	155.685521	52.587713
3227.287759	158.148119	52.592717
3226.729918	147.163351	52.597722
3225.631996	157.652897	52.602727
3225.303956	155.353947	52.607732
3224.371957	154.645911	52.612737
3223.843898	154.279383	52.617741
3222.968238	154.907745	52.622746
3222.300784	154.243328	52.627751
3222.187698	154.768648	52.632756
3221.152970	158.191628	52.637761
3220.800312	157.683031	52.642765
3220.025427	148.708987	52.647770
3219.238398	157.652163	52.652775
3218.812569	145.640260	52.657780
3217.762230	156.122467	52.662785
3217.409260	148.272764	52.667789
3217.428312	147.059625	52.672794
3216.630497	152.645109	52.677799
3215.757354	150.811517	52.682804
3214.678233	150.829655	52.687809
3214.522863	155.629213	52.692813
3214.156912	150.836531	52.697818
3212.657805	155.489482	52.702823
3211.968495	151.006644	52.707828
3211.648825	151.050953	52.712833
3210.839990	154.792571	52.717837
3210.471738	149.259378	52.722842
3209.577883	157.668581	52.727847
3209.352626	149.255098	52.732852
3208.731634	158.916339	52.737857
3208.244847	150.825426	52.742861
3207.096525	146.100491	52.747866
3206.179988	146.697945	52.752871
3205.825807	142.832447	52.757876
3205.575275	139.157658	52.762881
3204.465540	137.741455	52.767885
3203.792713	142.867829	52.772890
3203.315005	144.828702	52.777895
3203.053142	147.409922	52.782900
3201.791307	146.409695	52.787905
3201.742231	151.149645	52.792909
3201.138018	152.694378	52.797914
3199.795082	154.514526	52.802919
3199.142916	147.586714	52.807924
3198.400701	152.296667	52.812929
3197.920026	155.185659	52.817933
3198.032070	145.045247	52.822938
3196.980125	144.440996	52.827943
3196.010879	151.164561	52.832948
3195.173803	160.807064	52.837953
3194.898979	152.737964	52.842957
3194.361563	151.189246	52.847962
3193.188628	150.966053	52.852967
3193.439163	145.558851	52.857972
3192.255408	150.661206	52.862977
3191.403592	140.137193	52.867981
3191.010145	137.806398	52.872986
3190.403586	144.259975	52.877991
3190.017472	139.454955	52.882996
3188.941724	152.659994	52.888001
3187.919511	146.342894	52.893005
3187.422613	138.008592	52.898010
3187.124707	150.429040	52.903015
3186.193483	147.352114	52.908020
3185.867335	148.313301	52.913025
3185.201445	153.940984	52.918029
3184.452619	148.543076	52.923034
3183.498858	150.958697	52.928039
3183.650634	146.914391	52.933044
3183.081010	138.005159	52.938049
3182.439362	146.991780	52.943053
3181.520394	143.462377	52.948058
3180.173058	147.914933	52.953063
3179.579930	148.240037	52.958068
3178.750930	143.796467	52.963073
3178.414164	148.971217	52.968077
3177.921788	146.366409	52.973082
3177.021384	155.794734	52.978087
3176.771831	144.013246	52.983092
3176.179592	158.321051	52.988097
3175.784854	154.570637	52.993101
3175.288767	149.616646	52.998106
3173.887241	150.059734	53.003111
3173.189945	146.475880	53.008116
3172.153760	143.695963	53.013121
3171.577570	151.952604	53.018125
3171.419049	148.381698	53.023130
3170.599044	152.352197	53.028135
3170.130233	142.744440	53.033140
3168.689295	147.407195	53.038145
3169.029909	152.899626	53.043149
3168.499969	143.060345	53.048154
3167.692003	151.777759	53.053159
3166.974370	143.365910	53.058164
3166.211252	152.561573	53.063169
3164.840277	150.469236	53.068173
3164.825212	146.531987	53.073178
3164.280863	155.122656	53.078183
3164.062557	133.488556	53.083188
3163.168659	149.118124	53.088193
3162.434518	142.936942	53.093197
3162.088217	145.007205	53.098202
3160.827885	144.732636	53.103207
3160.117330	147.461962	53.108212
3159.195218	154.066560	53.113217
3158.404141	150.282420	53.118221
3158.414097	141.177460	53.123226
3157.728016	151.310465	53.128231
3157.265846	138.364547	53.133236
3156.494716	137.600618	53.138241
3155.624921	151.295062	53.143245
3154.880540	146.663753	53.148250
3153.999825	153.131412	53.153255
3153.987360	148.351764	53.158260
3153.427991	154.333083	53.163265
3152.793728	140.710004	53.168269
3152.087135	136.828146	53.173274
3151.057512	143.493344	53.178279
3150.429993	136.767778	53.183284
3149.744406	143.260120	53.188289
3148.727688	147.982239	53.193293
3148.405830	144.981204	53.198298
3147.090775	141.747239	53.203303
3147.280882	133.009391	53.208308
3146.578993	146.464754	53.213313
3146.192501	144.480923	53.218317
3145.657419	139.106506	53.223322
3144.663651	150.949543	53.228327
3144.353661	137.143173	53.233332
3143.284165	137.663353	53.238337
3142.444599	139.196986	53.243341
3141.672590	141.480902	53.248346
3140.675729	142.077485	53.253351
3140.038416	135.744770	53.258356
3139.492544	142.998355	53.263361
3139.138361	138.504063	53.268365
3139.108818	132.725519	53.273370
3137.845423	137.475572	53.278375
3137.374468	135.144209	53.283380
3136.598402	141.487804	53.288385
3135.687848	136.444771	53.293389
3135.279020	136.086696	53.298394
3134.148821	136.142391	53.303399
3134.269431	132.027627	53.308404
3133.558733	143.913082	53.313409
3133.123639	142.640173	53.318413
3132.036463	133.067819	53.323418
3130.741204	131.275971	53.328423
3130.970933	129.750135	53.333428
3130.460290	139.528692	53.338433
3130.189784	133.687505	53.343437
3129.063081	132.235533	53.348442
3127.566674	130.512790	53.353447
3127.800948	129.911023	53.358452
3127.069154	138.942252	53.363457
3126.217994	136.646642	53.368461
3125.573121	131.742163	53.373466
3124.589373	142.071676	53.378471
3124.022260	133.689780	53.383476
3123.243360	135.122263	53.388481
3122.496581	136.914775	53.393485
3122.172580	128.268324	53.398490
3121.141076	140.460030	53.403495
3120.851544	131.219544	53.408500
3119.698250	144.404670	53.413505
3119.766467	129.922258	53.418509
3119.729681	134.147349	53.423514
3117.938553	136.090668	53.428519
3117.447427	128.238149	53.433524
3117.299397	132.614480	53.438529
3116.215401	128.128050	53.443533
3115.706361	129.019831	53.448538
3115.223489	132.121563	53.453543
3114.850257	130.171787	53.458548
3113.424831	133.437326	53.463553
3112.132285	134.398244	53.468557
3112.422601	133.380726	53.473562
3111.802797	135.998235	53.478567
3111.454218	131.230629	53.483572
3110.898164	133.673434	53.488577
3109.592915	130.941873	53.493581
3108.741599	133.558676	53.498586
3108.205153	137.895586	53.503591
3107.773467	127.634943	53.508596
3107.290867	133.448011	53.513601
3106.843467	130.062653	53.518605
3105.774642	127.592664	53.523610
3104.276995	133.552324	53.528615
3104.304293	132.044101	53.533620
3103.871192	132.244767	53.538625
3103.125988	131.435363	53.543629
3102.908490	133.113366	53.548634
3101.976523	136.811688	53.553639
3101.712659	125.689498	53.558644
3100.152030	135.763900	53.563649
3099.407688	137.742310	53.568653
3099.694290	131.087534	53.573658
3098.514046	138.065833	53.578663
3097.953552	136.052924	53.583668
3096.991940	145.294342	53.588673
3096.331745	133.134628	53.593677
3096.036322	134.014780	53.598682
3095.412774	133.588003	53.603687
3094.578981	130.102092	53.608692
3093.410921	138.858530	53.613697
3093.249485	136.541785	53.618701
3093.026644	132.327420	53.623706
3092.044338	138.924934	53.628711
3090.986335	136.300338	53.633716
3089.843922	135.866692	53.638721
3089.759718	133.944110	53.643725
3089.359012	131.520226	53.648730
3088.922773	135.711334	53.653735
3088.060233	137.717836	53.658740
3087.785776	139.582014	53.663745
3086.638938	140.995661	53.668749
3086.230939	124.228236	53.673754
3084.918827	131.817209	53.678759
3084.730979	134.683011	53.683764
3084.310807	127.572699	53.688769
3082.893779	133.263988	53.693773
3082.900232	132.558650	53.698778
3081.989516	139.698919	53.703783
3081.771194	130.934944	53.708788
3080.627555	132.927899	53.713793
3079.376697	132.599625	53.718797
3079.533864	124.663579	53.723802
3078.989823	132.487623	53.728807
3078.262004	125.670662	53.733812
3077.145695	135.459548	53.738817
3076.873612	142.867269	53.743821
3076.235828	131.861468	53.748826
3075.004282	138.298680	53.753831
3074.946056	124.869702	53.758836
3074.448923	134.910808	53.763841
3073.212894	130.246686	53.768845
3072.837640	129.038952	53.773850
3071.938699	135.178154	53.778855
3071.844966	132.238015	53.783860
3071.113159	132.317621	53.788865
3070.098388	133.560681	53.793869
3069.337755	129.292556	53.798874
3068.587097	139.549480	53.803879
3068.306094	127.273672	53.808884
3067.350604	135.108416	53.813889
3066.884061	133.185245	53.818893
3066.391410	125.070109	53.823898
3065.441899	139.816691	53.828903
3065.011627	129.021352	53.833908
3064.321698	131.305066	53.838913
3063.715406	134.516308	53.843917
3063.472685	132.469632	53.848922
3062.612749	142.748388	53.853927
3062.130539	131.691140	53.858932
3061.130893	132.067560	53.863937
3059.439909	131.405557	53.868941
3059.880164	132.171452	53.873946
3059.334960	137.604835	53.878951
3058.225011	135.802655	53.883956
3057.332698	135.256415	53.888961
3056.623609	135.837787	53.893965
3057.016619	128.725105	53.898970
3055.617616	135.568292	53.903975
3055.011934	123.732825	53.908980
3054.300605	123.813277	53.913985
3053.300776	125.341147	53.918989
3053.009267	118.109783	53.923994
3052.217416	129.657391	53.928999
3052.119217	113.471378	53.934004
3051.156084	121.933854	53.939009
3050.726680	125.989980	53.944013
3050.403487	125.906219	53.949018
3049.559121	127.819621	53.954023
3048.747557	123.183239	53.959028
3047.802969	123.596831	53.964033
3046.404623	118.799011	53.969037
3046.282758	117.148519	53.974042
3045.891699	127.428857	53.979047
3045.292593	120.979112	53.984052
3044.514892	125.461059	53.989057
3043.869885	112.047495	53.994061
3043.375333	123.505221	53.999066
3042.837763	131.767095	54.004071
3042.178462	125.530525	54.009076
3041.429872	127.600453	54.014081
3040.781830	128.242051	54.019085
3040.269088	130.642723	54.024090
3038.786535	134.996040	54.029095
3037.920559	126.423265	54.034100
3037.900941	137.216441	54.039105
3037.604036	136.893325	54.044109
3036.491014	131.791361	54.049114
3035.363878	137.666015	54.054119
3034.879214	122.127071	54.059124
3035.093921	124.959216	54.064129
3033.857455	126.378713	54.069133
3033.344477	124.932022	54.074138
3032.297414	129.162768	54.079143
3032.099095	125.665781	54.084148
3031.450457	131.003154	54.089153
3030.525630	135.136438	54.094157
3030.365262	129.977085	54.099162
3029.931421	130.732474	54.104167
3028.857432	123.044304	54.109172
3027.527828	124.665633	54.114177
3027.374358	135.919826	54.119181
3026.814272	126.758744	54.124186
3025.574560	125.198609	54.129191
3025.134033	129.099141	54.134196
3025.105842	125.045729	54.139201
3024.160631	122.830944	54.144205
3023.210159	122.734768	54.149210
3022.877379	122.918692	54.154215
3022.500449	123.419232	54.159220
3021.862309	118.106660	54.164225
3021.106577	128.834960	54.169229
3020.059848	121.262922	54.174234
3018.740361	134.342237	54.179239
3018.982473	126.227472	54.184244
3018.089758	123.141635	54.189249
3016.982573	125.316656	54.194253
3016.976668	127.542303	54.199258
3016.097800	130.347373	54.204263
3015.445483	127.175458	54.209268
3015.017303	120.378756	54.214273
3014.152736	119.761074	54.219277
3013.708270	118.273074	54.224282
3012.995778	126.690359	54.229287
3012.900920	124.032646	54.234292
3011.870110	122.683917	54.239297
3010.236487	124.299964	54.244301
3009.950299	117.731231	54.249306
3009.112711	130.798460	54.254311
3009.203478	125.234626	54.259316
3008.063160	132.597681	54.264321
3006.995701	130.009850	54.269325
3007.050203	120.794281	54.274330
3006.327249	131.099755	54.279335
3005.799037	130.543411	54.284340
3005.046353	126.165784	54.289345
3004.266611	123.888781	54.294349
3004.042937	122.879356	54.299354
3003.477230	123.802144	54.304359
3002.588271	118.386387	54.309364
3001.191303	125.659877	54.314369
3000.403993	128.199046	54.319373
3000.162799	120.374893	54.324378
2999.507785	126.904247	54.329383
2999.253878	119.952246	54.334388
2998.538468	120.824038	54.339393
2997.959847	132.548760	54.344397
2997.682272	120.931578	54.349402
2996.790930	119.979798	54.354407
2995.350159	120.116616	54.359412
2994.664193	118.389629	54.364417
2994.020395	125.368634	54.369421
2994.187419	120.789641	54.374426
2993.076796	118.612207	54.379431
2992.360322	121.292031	54.384436
2991.987449	115.083105	54.389441
2991.360574	122.801303	54.394445
2990.731481	120.535269	54.399450
2990.128059	124.460479	54.404455
2988.880828	123.901086	54.409460
2988.254978	118.686285	54.414465
2987.041028	126.798876	54.419469
2987.266809	116.028424	54.424474
2986.171447	121.709759	54.429479
2985.818527	118.487873	54.434484
2985.437274	120.274777	54.439489
2984.791388	128.347138	54.444493
2984.114396	120.728902	54.449498
2983.390857	121.469063	54.454503
2982.799711	118.548010	54.459508
2981.825291	122.162022	54.464513
2981.008953	118.673151	54.469517
2980.293459	120.586644	54.474522
2979.657120	127.563586	54.479527
2979.081868	121.408584	54.484532
2978.906585	127.683466	54.489537
2978.095471	124.109230	54.494541
2977.940579	123.740141	54.499546
2976.833941	127.544112	54.504551
2975.562471	132.427014	54.509556
2974.394870	125.438916	54.514561
2974.795399	122.473531	54.519565
2974.241738	119.430420	54.524570
2973.083534	135.160398	54.529575
2972.579880	124.544985	54.534580
2972.085577	126.128189	54.539585
2971.411560	119.277585	54.544589
2970.842642	117.720858	54.549594
2970.394481	123.444358	54.554599
2969.089157	127.771744	54.559604
2968.209396	128.510183	54.564609
2967.521956	126.231228	54.569613
2967.747366	126.242797	54.574618
2966.740998	131.833537	54.579623
2965.701694	121.100457	54.584628
2965.465753	122.960028	54.589633
2964.578608	124.169454	54.594637
2964.549649	114.459747	54.599642
2963.893274	128.600057	54.604647
2963.062244	121.121039	54.609652
2961.881060	119.529602	54.614657
2960.634675	122.678526	54.619661
2960.512867	119.719903	54.624666
2959.889919	123.265962	54.629671
2959.495524	118.352657	54.634676
2959.189038	109.453781	54.639681
2958.291595	114.755909	54.644685
2958.164268	117.885307	54.649690
2956.899626	118.951616	54.654695
2956.163031	119.121658	54.659700
2955.202116	125.582107	54.664705
2954.439710	126.302072	54.669709
2954.559943	116.737786	54.674714
2953.686303	121.481654	54.679719
2953.016376	119.596015	54.684724
2952.514922	120.209020	54.689729
2951.295443	124.176747	54.694733
2950.522200	128.484261	54.699738
2949.774835	121.901978	54.704743
2949.185076	120.124215	54.709748
2948.939293	120.978127	54.714753
2948.152286	121.908344	54.719757
2948.205167	119.194600	54.724762
2947.112266	125.869441	54.729767
2946.899184	126.810526	54.734772
2945.578087	123.541335	54.739777
2944.624155	120.637285	54.744781
2943.987863	116.163205	54.749786
2943.480957	120.515991	54.754791
2942.984166	116.378851	54.759796
2942.809091	119.458779	54.764801
2941.789984	121.112721	54.769805
2941.283393	118.650106	54.774810
2940.105497	118.133348	54.779815
2939.300009	112.136120	54.784820
2938.811275	116.145939	54.789825
2938.086362	112.225018	54.794829
2937.845574	106.181816	54.799834
2936.954332	117.043394	54.804839
2936.650101	110.152503	54.809844
2936.435723	102.008793	54.814849
2935.167961	118.754162	54.819853
2934.602727	109.659908	54.824858
2934.059094	113.398853	54.829863
2933.661695	116.045470	54.834868
2932.295814	118.935353	54.839873
2930.476015	123.292244	54.844877
2930.875743	113.921376	54.849882
2930.765211	129.377183	54.854887
2929.671798	125.259898	54.859892
2928.919320	121.664205	54.864897
2928.209586	126.202045	54.869901
2927.824569	118.891941	54.874906
2927.050515	122.940259	54.879911
2926.550699	121.498435	54.884916
2926.174945	116.591423	54.889921
2925.229545	117.010699	54.894925
2924.290732	109.572220	54.899930
2923.453039	124.973082	54.904935
2922.945600	124.193728	54.909940
2922.573124	121.488728	54.914945
2921.806864	121.408061	54.919949
2921.367998	117.772591	54.924954
2920.757925	116.640524	54.929959
2920.157898	112.980492	54.934964
2919.323720	122.755905	54.939969
2918.256735	119.367510	54.944973
2918.139548	120.836534	54.949978
2917.318392	118.703594	54.954983
2917.248391	116.688595	54.959988
2915.631982	118.956971	54.964993
2914.746835	112.275485	54.969997
2914.364955	117.010315	54.975002
2913.647477	125.063332	54.980007
2912.860157	119.198393	54.985012
2912.649123	116.442122	54.990017
2912.107189	117.535325	54.995021
2911.811732	113.352337	55.000026
2910.967215	116.395092	55.005031
2910.511804	112.809819	55.010036
2909.356192	119.319331	55.015041
2908.168679	117.557677	55.020045
2907.780796	111.397118	55.025050
2906.994028	119.373555	55.030055
2906.733337	108.894272	55.035060
2906.266834	118.876052	55.040065
2906.018578	108.429774	55.045069
2904.491798	108.764071	55.050074
2903.593657	110.459318	55.055079
2903.194671	114.139204	55.060084
2902.490465	111.905757	55.065089
2901.771263	116.127854	55.070093
2901.511014	112.960401	55.075098
2900.943836	113.141365	55.080103
2900.679413	115.813019	55.085108
2899.405672	111.053554	55.090113
2898.417592	112.566019	55.095117
2898.084567	113.928249	55.100122
2897.309654	118.806035	55.105127
2896.812922	117.523947	55.110132
2896.569750	107.525606	55.115137
2895.577226	119.859061	55.120141
2894.901538	107.805878	55.125146
2894.118435	111.121947	55.130151
2893.567186	115.506389	55.135156
2892.891472	114.078447	55.140161
2892.136042	109.801180	55.145165
2891.630959	107.852643	55.150170
2890.188954	112.979034	55.155175
2889.734958	110.577701	55.160180
2889.242112	103.435244	55.165185
2888.429336	110.100502	55.170189
2887.993110	106.970625	55.175194
2887.605640	117.000080	55.180199
2887.209586	120.516445	55.185204
2887.080515	112.853144	55.190209
2886.046169	120.955181	55.195213
2885.172773	112.613055	55.200218
2883.746883	109.497973	55.205223
2883.160608	107.298058	55.210228
2882.860921	113.333277	55.215233
2882.041853	117.695203	55.220237
2881.836427	108.769594	55.225242
2881.064210	111.612107	55.230247
2879.913386	105.922588	55.235252
2879.243261	111.225347	55.240257
2878.667012	116.628114	55.245261
2878.221210	116.816757	55.250266
2877.763496	117.488212	55.255271
2877.436827	112.853469	55.260276
2876.881449	119.010148	55.265281
2875.739688	118.821561	55.270285
2874.691778	119.260337	55.275290
2873.965918	123.641072	55.280295
2873.592326	120.978898	55.285300
2873.082158	115.258835	55.290305
2872.454009	118.157252	55.295309
2872.166233	114.627411	55.300314
2870.810440	113.128992	55.305319
2870.027412	108.018049	55.310324
2869.634666	113.406822	55.315329
2868.784984	122.435302	55.320333
2868.463145	113.269857	55.325338
2867.930133	118.596553	55.330343
2867.481822	115.792813	55.335348
2866.899180	113.366889	55.340353
2865.684184	116.387310	55.345357
2865.204987	112.405855	55.350362
2864.405887	114.440224	55.355367
2863.712703	111.820830	55.360372
2863.266507	106.802319	55.365377
2861.949141	117.765936	55.370381
2861.198582	101.898693	55.375386
2861.067811	112.616489	55.380391
2860.787049	111.496436	55.385396
2860.268266	114.326427	55.390401
2859.546299	111.911290	55.395405
2858.791232	113.298678	55.400410
2857.290933	115.219602	55.405415
2856.806413	108.436900	55.410420
2856.373538	110.584727	55.415425
2855.673048	108.180920	55.420429
2855.972819	104.951315	55.425434
2855.006592	108.001850	55.430439
2853.786780	112.576736	55.435444
2852.883857	105.767651	55.440449
2851.942155	109.578184	55.445453
2851.712488	112.546259	55.450458
2851.344782	113.554823	55.455463
2850.784617	117.317519	55.460468
2850.494053	110.905079	55.465473
2849.429869	118.317106	55.470477
2848.542066	107.494232	55.475482
2847.659025	104.750583	55.480487
2847.183656	103.818129	55.485492
2846.817363	104.650799	55.490497
2846.074519	111.989352	55.495501
2845.454556	107.818806	55.500506
2844.422426	102.973462	55.505511
2843.659661	111.396179	55.510516
2842.834526	108.935520	55.515521
2842.298311	113.202135	55.520525
2842.235523	110.057386	55.525530
2841.760079	114.300984	55.530535
2841.182457	112.027754	55.535540
2840.231853	115.100096	55.540545
2839.022863	109.759992	55.545549
2838.548301	104.221742	55.550554
2837.999863	111.901270	55.555559
2837.796564	113.649083	55.560564
2836.723053	107.973993	55.565569
2835.580909	111.974308	55.570573
2835.126736	104.666571	55.575578
2834.548571	107.638155	55.580583
2834.074934	112.098937	55.585588
2833.529433	105.264296	55.590593
2833.091903	105.597576	55.595597
2832.583498	99.968800	55.600602
2831.324418	101.642456	55.605607
2830.663252	100.778072	55.610612
2830.043995	95.613099	55.615617
2829.239300	104.063503	55.620621
2829.343754	94.228789	55.625626
2827.903309	96.384613	55.630631
2826.533611	98.531504	55.635636
2826.879576	100.212677	55.640641
2826.060943	114.515302	55.645645
2825.564440	92.669563	55.650650
2824.784253	101.906018	55.655655
2824.137167	100.719897	55.660660
2824.073411	98.073854	55.665665
2823.004497	96.444711	55.670669
2822.472585	92.484908	55.675674
2821.486496	91.079629	55.680679
2821.101986	101.699863	55.685684
2820.492224	95.528298	55.690689
2818.696987	106.847130	55.695693
2818.261015	99.179455	55.700698
2818.456564	101.081331	55.705703
2817.615370	97.258463	55.710708
2816.879249	92.788841	55.715713
2816.226740	100.833114	55.720717
2815.901982	93.946937	55.725722
2815.210475	102.220501	55.730727
2813.917772	99.068864	55.735732
2813.470718	92.596736	55.740737
2812.555628	104.018159	55.745741
2812.424772	98.974971	55.750746
2811.908611	103.716565	55.755751
2811.341143	103.592464	55.760756
2810.669581	95.653224	55.765761
2809.314882	97.859527	55.770765
2808.924388	100.670356	55.775770
2808.353610	95.492758	55.780775
2807.650600	93.591877	55.785780
2807.430171	89.958565	55.790785
2805.939852	101.906972	55.795789
2805.400657	95.395332	55.800794
2804.947667	97.948428	55.805799
2804.289731	98.990414	55.810804
2804.142928	95.842661	55.815809
2803.293722	107.179408	55.820813
2802.253647	96.823488	55.825818
2801.312248	101.356321	55.830823
2800.359173	102.449935	55.835828
2800.117959	97.313113	55.840833
2799.524376	103.476319	55.845837
2799.870430	95.681701	55.850842
2799.111789	96.980103	55.855847
2798.099331	101.561396	55.860852
2797.478924	97.808161	55.865857
2796.516112	103.926319	55.870861
2795.502789	99.757885	55.875866
2795.024591	105.255995	55.880871
2794.038079	98.685418	55.885876
2793.218933	97.387791	55.890881
2792.420029	106.561135	55.895885
2792.795188	92.695404	55.900890
2792.028117	97.865133	55.905895
2791.196574	101.543163	55.910900
2791.098231	94.737104	55.915905
2790.428765	97.548247	55.920909
2789.466314	101.871528	55.925914
2788.685505	99.097787	55.930919
2787.924322	100.736089	55.935924
2786.643032	95.848875	55.940929
2786.103551	104.972352	55.945933
2785.797635	95.466325	55.950938
2784.993836	98.769756	55.955943
2784.197033	95.542842	55.960948
2784.050246	99.059233	55.965953
2783.325293	98.508907	55.970957
2783.191240	96.063166	55.975962
2781.783647	97.083682	55.980967
2780.768366	98.761861	55.985972
2780.489812	94.636000	55.990977
2779.565818	102.220244	55.995981
2779.412522	97.720089	56.000986
2779.029808	92.247072	56.005991
2778.249123	93.249648	56.010996
2777.549903	93.575556	56.016001
2776.147679	96.114058	56.021005
2776.160012	95.264434	56.026010
2775.562138	86.415007	56.031015
2774.972876	100.939327	56.036020
2774.085988	96.563373	56.041025
2772.965729	100.148256	56.046029
2772.412496	93.584944	56.051034
2771.992554	96.579222	56.056039
2771.362024	96.909969	56.061044
2771.119485	92.047318	56.066049
2769.839863	108.050258	56.071053
2768.908867	95.594318	56.076058
2768.328442	99.521131	56.081063
2767.787727	101.974754	56.086068
2767.301676	96.550583	56.091073
2766.846319	94.856844	56.096077
2766.766452	99.418475	56.101082
2765.697554	97.428168	56.106087
2764.729418	97.382027	56.111092
2764.128025	90.016973	56.116097
2763.800306	97.991918	56.121101
2763.109654	92.892447	56.126106
2761.629940	96.436140	56.131111
2760.900624	102.622152	56.136116
2760.140525	85.549913	56.141121
2759.851949	94.540897	56.146125
2759.986946	97.711896	56.151130
2758.840969	94.379279	56.156135
2758.444093	102.947081	56.161140
2758.068597	96.029322	56.166145
2756.610567	104.004443	56.171149
2756.161431	103.652891	56.176154
2755.507123	100.260709	56.181159
2755.157033	101.351527	56.186164
2754.316626	97.238809	56.191169
2753.055117	98.479487	56.196173
2752.459866	91.130359	56.201178
2752.200015	95.140532	56.206183
2751.384393	101.448661	56.211188
2751.286397	95.125295	56.216193
2750.464367	97.492795	56.221197
2749.315889	91.370297	56.226202
2748.821988	90.758775	56.231207
2748.256449	92.216407	56.236212
2747.911066	96.759474	56.241217
2747.479095	99.040174	56.246221
2746.669566	93.708795	56.251226
2745.652815	90.413698	56.256231
2744.687652	90.890457	56.261236
2744.359752	91.874459	56.266241
2743.545116	98.526619	56.271245
2742.558333	93.737891	56.276250
2741.545738	92.956876	56.281255
2741.419286	90.743516	56.286260
2740.941507	94.017278	56.291265
2740.066872	102.522271	56.296269
2739.555455	95.649851	56.301274
2739.519323	98.820100	56.306279
2738.870633	100.004982	56.311284
2737.904566	89.223159	56.316289
2736.633619	101.674457	56.321293
2736.060548	99.156130	56.326298
2735.386573	99.820745	56.331303
2735.251795	102.263404	56.336308
2735.065965	92.008199	56.341313
2733.610336	104.733032	56.346317
2733.251447	98.083219	56.351322
2732.641371	93.945741	56.356327
2731.892218	97.842976	56.361332
2730.928894	87.996186	56.366337
2730.243907	96.595072	56.371341
2729.812777	89.696697	56.376346
2729.196888	95.032030	56.381351
2728.370778	95.110431	56.386356
2728.155710	95.192938	56.391361
2727.089383	97.268260	56.396365
2726.699732	100.025265	56.401370
2726.334848	94.026986	56.406375
2725.195744	94.235857	56.411380
2724.127770	91.191486	56.416385
2723.111668	88.229825	56.421389
2722.673274	92.360513	56.426394
2722.054991	91.119352	56.431399
2721.431633	97.731318	56.436404
2721.306011	88.917229	56.441409
2720.733892	98.352193	56.446413
2720.595516	92.770711	56.451418
2719.647506	89.550314	56.456423
2718.395461	92.883396	56.461428
2717.863544	90.991572	56.466433
2717.016011	93.858024	56.471437
2716.760094	84.503332	56.476442
2716.178705	92.888725	56.481447
2714.883260	97.326562	56.486452
2714.840677	85.898230	56.491457
2713.781924	100.337406	56.496461
2713.548255	92.548333	56.501466
2713.164020	105.180429	56.506471
2711.936718	101.803303	56.511476
2711.402896	99.412871	56.516481
2710.420193	101.043258	56.521485
2710.009669	96.794307	56.526490
2708.823154	97.471930	56.531495
2707.813925	92.994143	56.536500
2707.684946	85.379410	56.541505
2707.091932	99.718452	56.546509
2706.504753	95.630351	56.551514
2706.103427	91.435487	56.556519
2705.297905	96.708107	56.561524
2705.070841	95.828747	56.566529
2704.352640	98.008773	56.571533
2703.390135	94.604941	56.576538
2702.581512	100.856221	56.581543
2701.828677	90.192692	56.586548
2701.724232	90.915481	56.591553
2700.869040	97.691020	56.596557
2699.734387	90.407261	56.601562
2699.028908	84.715489	56.606567
2698.648263	90.001138	56.611572
2698.214945	92.862314	56.616577
2697.528641	94.691504	56.621581
2697.322267	93.192838	56.626586
2696.226065	91.710092	56.631591
2695.209788	96.060346	56.636596
2694.892491	92.806353	56.641601
2694.196012	102.107449	56.646605
2693.220859	95.031287	56.651610
2692.203875	94.950878	56.656615
2691.401908	92.324846	56.661620
2690.901960	91.184247	56.666625
2690.935590	86.172560	56.671629
2690.354031	82.905716	56.676634
2689.907648	80.402057	56.681639
2689.063282	96.204277	56.686644
2688.624859	93.508209	56.691649
2687.539325	97.386766	56.696653
2686.903750	88.714321	56.701658
2686.443630	93.059901	56.706663
2685.463181	96.503666	56.711668
2684.413548	80.952481	56.716673
2683.749135	91.613442	56.721677
2683.241127	92.965328	56.726682
2683.077444	92.619856	56.731687
2682.463761	96.300129	56.736692
2682.502128	88.982440	56.741697
2681.125693	89.072420	56.746701
2679.884824	95.022991	56.751706
2679.982951	94.659608	56.756711
2679.114961	100.332897	56.761716
2678.095139	92.802548	56.766721
2677.380380	93.654924	56.771725
2676.696601	94.207145	56.776730
2676.395702	94.103016	56.781735
2675.790552	96.097541	56.786740
2675.126999	90.387553	56.791745
2674.000404	91.759523	56.796749
2673.311312	89.006046	56.801754
2672.603746	90.360072	56.806759
2672.277028	95.911627	56.811764
2672.391612	84.582748	56.816769
2671.179612	92.698580	56.821773
2670.281582	88.212847	56.826778
2669.077827	78.982292	56.831783
2668.539385	98.231055	56.836788
2668.675890	91.707750	56.841793
2667.718466	89.811300	56.846797
2667.093595	90.042410	56.851802
2666.341258	94.595437	56.856807
2665.285144	93.083346	56.861812
2664.864181	93.099606	56.866817
2664.455611	98.224642	56.871821
2664.266628	88.790225	56.876826
2663.457297	91.159511	56.881831
2662.262101	85.922892	56.886836
2661.934193	87.617008	56.891841
2661.215987	88.419451	56.896845
2660.613185	88.878887	56.901850
2659.512056	88.351829	56.906855
2658.632794	94.507425	56.911860
2658.620292	86.917390	56.916865
2657.786953	90.116544	56.921869
2657.224533	91.798644	56.926874
2656.796293	91.817728	56.931879
2655.379329	84.211991	56.936884
2655.067973	89.929071	56.941889
2654.178426	91.713273	56.946893
2653.809521	87.790759	56.951898
2653.635930	86.085183	56.956903
2652.606067	90.072644	56.961908
2651.780769	89.575803	56.966913
2650.857896	91.997656	56.971917
2650.435636	91.263374	56.976922
2650.016921	87.758704	56.981927
2649.443522	95.061978	56.986932
2648.846488	92.685124	56.991937
2647.473116	93.695086	56.996941
2646.964274	87.680771	57.001946
2646.672026	86.074423	57.006951
2646.030743	89.990723	57.011956
2645.760640	82.616037	57.016961
2644.414190	96.482306	57.021965
2643.906108	87.541374	57.026970
2643.447864	86.274839	57.031975
2642.539391	90.008663	57.036980
2642.038194	87.215967	57.041985
2640.881690	91.141396	57.046989
2640.291002	95.437064	57.051994
2639.958318	80.703178	57.056999
2638.978832	87.591540	57.062004
2638.944804	90.850238	57.067009
2638.344615	97.039444	57.072013
2637.036202	97.055046	57.077018
2636.442477	96.872295	57.082023
2635.778859	91.627704	57.087028
2635.560457	86.196091	57.092033
2634.977265	101.415266	57.097037
2634.190534	97.508125	57.102042
2633.035403	103.811539	57.107047
2632.377330	99.606493	57.112052
2632.106715	95.472973	57.117057
2631.370343	94.725284	57.122061
2631.142314	89.103480	57.127066
2630.402651	87.987287	57.132071
2628.743543	104.615214	57.137076
2628.672344	91.578146	57.142081
2628.178473	94.797429	57.147085
2627.870694	85.573585	57.152090
2626.414117	91.686165	57.157095
2625.663998	89.867571	57.162100
2625.219160	78.589332	57.167105
2624.666116	88.463909	57.172109
2624.353045	87.755173	57.177114
2624.042604	93.135003	57.182119
2622.594545	94.832322	57.187124
2622.182312	94.105801	57.192129
2621.185482	102.879972	57.197133
2620.624431	98.587686	57.202138
2620.669886	93.836470	57.207143
2619.328361	89.456955	57.212148
2618.772368	90.341406	57.217153
2617.816306	91.142674	57.222157
2617.160723	89.092007	57.227162
2617.088865	94.441710	57.232167
2615.997596	93.969816	57.237172
2615.506122	87.433870	57.242177
2614.928741	86.791237	57.247181
2613.874832	87.561864	57.252186
2613.591566	95.163689	57.257191
2612.721937	93.536442	57.262196
2612.778492	87.720339	57.267201
2612.126343	99.172998	57.272205
2610.948759	92.748812	57.277210
2610.274884	90.183790	57.282215
2609.589483	97.451741	57.287220
2609.004432	87.015337	57.292225
2608.198314	95.100082	57.297229
2607.634843	89.170108	57.302234
2607.191861	92.524373	57.307239
2606.252842	95.365821	57.312244
2605.846287	95.348440	57.317249
2605.117072	96.741305	57.322253
2603.956585	90.304331	57.327258
2603.711397	91.887996	57.332263
2603.232079	92.646450	57.337268
2602.440449	86.286945	57.342273
2601.076226	90.501303	57.347277
2600.525928	96.481461	57.352282
2600.233458	84.598510	57.357287
2599.582323	100.587167	57.362292
2599.634599	90.367855	57.367297
2598.548364	92.488442	57.372301
2597.422013	89.779726	57.377306
2596.847288	88.443505	57.382311
2596.338381	93.775556	57.387316
2595.847607	82.030714	57.392321
2595.268368	87.053875	57.397325
2594.130715	92.726296	57.402330
2593.143949	86.145160	57.407335
2592.452164	100.252799	57.412340
2592.205366	90.817223	57.417345
2592.195644	95.754475	57.422349
2591.710559	89.049681	57.427354
2591.092820	90.378097	57.432359
2589.669977	83.804407	57.437364
2589.620386	91.975736	57.442369
2588.478162	95.853735	57.447373
2587.250903	91.175230	57.452378
2586.936615	92.889521	57.457383
2586.147168	92.582740	57.462388
2585.869711	83.647394	57.467393
2585.455100	87.456661	57.472397
2584.889286	88.913960	57.477402
2583.879274	85.954051	57.482407
2582.678590	96.113421	57.487412
2582.881446	81.546935	57.492417
2581.801619	86.120032	57.497421
2581.400146	91.962251	57.502426
2580.328033	82.910921	57.507431
2579.454766	88.646300	57.512436
2579.140649	89.633085	57.517441
2578.692901	92.349107	57.522445
2578.410542	91.181979	57.527450
2577.466513	93.705351	57.532455
2576.122559	91.349619	57.537460
2575.613753	87.192092	57.542465
2575.258805	88.661894	57.547469
2574.724782	92.669203	57.552474
2574.475516	86.682364	57.557479
2573.067672	92.974512	57.562484
2572.581265	93.380902	57.567489
2571.279825	88.053132	57.572493
2570.719482	87.130495	57.577498
2570.604707	84.772257	57.582503
2569.875124	87.571984	57.587508
2569.696478	89.742282	57.592513
2568.878864	86.421074	57.597517
2568.071017	92.018565	57.602522
2567.797507	88.511581	57.607527
2566.501068	94.494169	57.612532
2565.554991	96.796453	57.617537
2564.705618	90.465377	57.622541
2564.445755	91.624066	57.627546
2564.114037	84.073613	57.632551
2563.422402	86.579100	57.637556
2563.273158	87.733482	57.642561
2562.531050	92.500683	57.647565
2561.278042	98.828732	57.652570
2560.641410	97.261133	57.657575
2559.935604	101.769507	57.662580
2559.644665	90.747191	57.667585
2558.470119	100.830653	57.672589
2557.447603	90.067611	57.677594
2557.194903	95.002190	57.682599
2556.797684	93.501027	57.687604
2556.711291	83.068202	57.692609
2556.014708	86.452006	57.697613
2555.059768	90.732583	57.702618
2554.772856	81.575840	57.707623
2553.145002	85.929615	57.712628
2552.409820	83.184431	57.717633
2551.578814	92.146167	57.722637
2551.086426	81.237243	57.727642
2550.689859	85.749587	57.732647
2550.282317	89.678827	57.737652
2550.271025	87.577627	57.742657
2548.822932	87.240957	57.747661
2547.984784	92.593769	57.752666
2547.529737	90.725927	57.757671
2546.848344	89.495182	57.762676
2546.348577	91.407362	57.767681
2544.984110	91.231653	57.772685
2544.079519	94.329321	57.777690
2544.204869	98.732312	57.782695
2543.298403	103.378015	57.787700
2543.056104	92.907104	57.792705
2542.042637	94.375807	57.797709
2541.966850	92.729302	57.802714
2541.781543	84.568841	57.807719
2540.156788	101.443131	57.812724
2540.043669	90.433048	57.817729
2538.651511	88.438845	57.822733
2537.598035	95.191849	57.827738
2537.042740	96.026058	57.832743
2536.617276	88.344402	57.837748
2536.472496	86.662720	57.842753
2536.056536	95.598106	57.847757
2535.201110	93.602141	57.852762
2535.261773	89.972899	57.857767
2533.422809	95.533918	57.862772
2532.895048	91.363057	57.867777
2532.216227	90.048983	57.872781
2531.414501	91.473594	57.877786
2530.668975	87.640349	57.882791
2529.643267	97.363640	57.887796
2529.408718	84.107029	57.892801
2528.817519	93.912739	57.897805
2528.237525	89.828570	57.902810
2528.291798	85.974245	57.907815
2527.416935	89.936408	57.912820
2526.336262	87.817117	57.917825
2525.643023	93.932238	57.922829
2524.778983	93.854132	57.927834
2524.567350	89.563308	57.932839
2524.030508	90.745273	57.937844
2523.027345	88.769437	57.942849
2522.335338	95.796554	57.947853
2521.761421	87.566352	57.952858
2521.289903	80.061123	57.957863
2520.641159	96.397902	57.962868
2519.243493	92.568785	57.967873
2519.006156	92.162491	57.972877
2518.030671	88.555662	57.977882
2517.815457	93.923949	57.982887
2517.418733	98.451323	57.987892
2517.070692	91.566406	57.992897
2515.664725	89.802326	57.997901
2514.922295	95.659024	58.002906
2514.730859	91.467770	58.007911
2514.009225	92.123190	58.012916
2513.324053	84.944609	58.017921
2512.178573	89.244346	58.022925
2511.557980	91.547436	58.027930
2511.234148	90.698840	58.032935
2510.317959	91.963424	58.037940
2510.262725	89.229495	58.042945
2509.381603	91.110168	58.047949
2508.415605	92.360768	58.052954
2508.182494	85.734091	58.057959
2507.391194	95.542435	58.062964
2506.273221	98.480412	58.067969
2505.434597	101.911007	58.072973
2504.881021	95.734233	58.077978
2504.862982	92.496198	58.082983
2503.991846	100.551805	58.087988
2503.668212	91.141615	58.092993
2502.726458	86.387086	58.097997
2501.588312	82.428742	58.103002
2501.347842	87.126367	58.108007
2500.676443	85.774319	58.113012
2500.099620	83.995983	58.118017
2498.946786	88.841303	58.123021
2498.177671	89.281823	58.128026
2497.750907	84.026370	58.133031
2496.818865	84.081864	58.138036
2496.713675	82.042112	58.143041
2496.270785	84.503499	58.148045
2495.850937	91.179754	58.153050
2494.995145	88.547959	58.158055
2494.358296	92.837316	58.163060
2493.934756	94.237142	58.168065
2492.653314	88.312311	58.173069
2492.202454	83.544119	58.178074
2491.885382	79.320668	58.183079
2490.486674	87.940531	58.188084
2489.522867	78.223762	58.193089
2489.002990	80.797781	58.198093
2488.218046	85.477181	58.203098
2487.975030	88.376091	58.208103
2487.631622	85.105268	58.213108
2487.580970	82.743966	58.218113
2486.291077	82.544075	58.223117
2484.693999	83.025104	58.228122
2484.497044	79.613589	58.233127
2484.203193	85.030052	58.238132
2483.858579	89.927845	58.243137
2482.772890	84.579398	58.248141
2481.840778	84.851216	58.253146
2481.107654	83.134341	58.258151
2480.645076	91.943093	58.263156
2480.272571	96.253966	58.268161
2480.407269	85.453360	58.273165
2479.060931	95.529094	58.278170
2478.462616	79.174136	58.283175
2477.384009	89.438164	58.288180
2476.805019	82.282094	58.293185
2475.488697	84.738871	58.298189
2474.818660	82.759773	58.303194
2474.761672	85.295704	58.308199
2474.290393	87.993254	58.313204
2473.758888	89.256019	58.318209
2473.601517	82.374827	58.323213
2472.293623	85.081998	58.328218
2471.410697	80.056508	58.333223
2470.669735	80.698658	58.338228
2470.362584	82.274763	58.343233
2469.860769	80.448872	58.348237
2468.620361	89.209431	58.353242
2467.882589	81.788810	58.358247
2467.103173	83.742096	58.363252
2466.860537	71.820265	58.368257
2466.525507	82.046365	58.373261
2465.936162	75.534680	58.378266
2464.789922	81.249241	58.383271
2463.924983	74.831253	58.388276
2463.352097	81.862473	58.393281
2462.780040	80.174510	58.398285
2462.581437	83.838299	58.403290
2462.344346	81.703078	58.408295
2461.130144	82.483377	58.413300
2460.566170	76.023800	58.418305
2459.641614	81.891111	58.423309
2458.801172	84.002853	58.428314
2458.070944	69.754605	58.433319
2457.099856	87.060267	58.438324
2456.721055	82.800795	58.443329
2456.554999	81.309460	58.448333
2455.862518	80.973883	58.453338
2455.536775	75.208946	58.458343
2454.316032	85.640559	58.463348
2453.578853	71.724671	58.468353
2453.284057	73.286426	58.473357
2452.597784	82.065526	58.478362
2452.304364	80.084800	58.483367
2450.794828	79.335913	58.488372
2450.031136	82.402001	58.493377
2449.735134	77.846542	58.498381
2449.028148	83.132332	58.503386
2449.078268	77.747984	58.508391
2447.491084	88.376853	58.513396
2446.785554	77.023622	58.518401
2446.361307	78.029637	58.523405
2446.012763	83.952407	58.528410
2445.679885	84.966484	58.533415
2444.131996	83.328528	58.538420
2443.732477	79.012209	58.543425
2443.250562	90.148001	58.548429
2442.447349	83.839062	58.553434
2442.347556	81.618790	58.558439
2440.910236	85.340431	58.563444
2440.447042	83.379260	58.568449
2440.000610	82.964512	58.573453
2439.296432	88.430607	58.578458
2438.757394	85.997288	58.583463
2437.566815	88.863613	58.588468
2437.152737	82.769579	58.593473
2436.762659	80.562626	58.598477
2436.038446	80.213136	58.603482
2435.409042	82.766808	58.608487
2434.355102	81.338075	58.613492
2433.620482	79.729618	58.618497
2433.224358	77.930659	58.623501
2432.379303	79.902672	58.628506
2432.652897	78.835097	58.633511
2431.201998	80.194669	58.638516
2430.183084	80.423312	58.643521
2429.743728	79.547502	58.648525
2429.443621	76.553484	58.653530
2428.994408	78.280585	58.658535
2427.277156	86.783217	58.663540
2427.140379	83.162476	58.668545
2426.779484	78.802056	58.673549
2426.057154	84.094023	58.678554
2425.709033	80.342450	58.683559
2424.806676	85.772170	58.688564
2423.794009	77.722795	58.693569
2423.244634	85.014068	58.698573
2422.776827	78.746073	58.703578
2422.704181	75.331861	58.708583
2421.180312	78.314777	58.713588
2420.641557	78.451455	58.718593
2420.070208	81.887277	58.723597
2419.649099	84.070216	58.728602
2418.910559	72.420282	58.733607
2417.856323	80.340224	58.738612
2417.254152	76.450123	58.743617
2416.606266	84.545317	58.748621
2415.749386	78.256220	58.753626
2415.791133	74.672850	58.758631
2414.397043	87.354424	58.763636
2413.660543	80.109249	58.768641
2413.155416	71.517985	58.773645
2412.388816	80.027408	58.778650
2412.637448	84.445226	58.783655
2412.081521	71.692003	58.788660
2410.808808	78.521971	58.793665
2409.851901	82.652511	58.798669
2409.132842	74.160586	58.803674
2408.686086	77.754308	58.808679
2408.214527	75.927988	58.813684
2407.830614	76.963028	58.818689
2406.527128	78.700018	58.823693
2405.850579	78.189230	58.828698
2405.531127	80.871480	58.833703
2404.603475	85.501080	58.838708
2404.637847	75.076841	58.843713
2403.442796	78.873112	58.848717
2402.428766	79.388284	58.853722
2401.848398	79.210380	58.858727
2401.623125	78.430990	58.863732
2401.256613	76.812491	58.868737
2400.810569	80.003869	58.873741
2399.151334	87.630566	58.878746
2399.066236	83.624818	58.883751
2398.272025	83.428612	58.888756
2397.998684	81.982465	58.893761
2396.986165	75.870769	58.898765
2395.742444	86.306317	58.903770
2395.538342	74.392118	58.908775
2395.084402	73.989710	58.913780
2394.727009	76.584504	58.918785
2393.738878	77.358528	58.923789
2392.862703	74.498143	58.928794
2392.489807	76.412322	58.933799
2392.035934	78.840066	58.938804
2391.294273	73.867413	58.943809
2390.257701	74.885765	58.948813
2389.595969	80.730642	58.953818
2389.346078	74.601045	58.958823
2387.968016	86.652667	58.963828
2387.467455	78.710337	58.968833
2386.889483	77.241281	58.973837
2386.077388	87.343301	58.978842
2385.963819	83.975559	58.983847
2385.468387	82.548440	58.988852
2384.667163	73.594139	58.993857
2383.810507	78.215153	58.998861
2383.068736	78.973106	59.003866
2382.344182	74.580140	59.008871
2381.509398	78.365339	59.013876
2380.703270	73.295951	59.018881
2379.965548	73.779670	59.023885
2379.134000	83.708968	59.028890
2379.204747	72.519066	59.033895
2378.491935	79.074099	59.038900
2378.059884	75.257939	59.043905
2377.344476	77.641196	59.048909
2376.084525	74.731966	59.053914
2375.814055	66.711618	59.058919
2375.095598	75.186757	59.063924
2374.885462	69.854417	59.068929
2373.639051	80.200821	59.073933
2372.832001	82.257919	59.078938
2372.556242	74.470570	59.083943
2371.892818	86.541308	59.088948
2371.571303	77.346699	59.093953
2371.016213	81.515112	59.098957
2369.501197	82.575805	59.103962
2368.965295	77.798490	59.108967
2368.796673	77.877015	59.113972
2367.998683	87.165863	59.118977
2366.944186	82.925627	59.123981
2366.108487	91.930015	59.128986
2365.892192	80.694852	59.133991
2365.036516	81.199531	59.138996
2364.635757	85.827855	59.144001
2364.143486	83.587858	59.149005
2363.014452	92.865817	59.154010
2362.523984	84.007584	59.159015
2361.792977	83.832154	59.164020
2361.286225	77.748454	59.169025
2360.970564	86.156303	59.174029
2360.083589	86.584233	59.179034
2359.419733	81.691828	59.184039
2358.645391	88.303965	59.189044
2358.274819	79.497074	59.194049
2356.928303	83.023607	59.199053
2356.108887	90.457370	59.204058
2355.838117	76.932659	59.209063
2355.248962	80.223113	59.214068
2354.602201	74.599525	59.219073
2354.023741	83.105202	59.224077
2353.355414	91.669669	59.229082
2352.374786	79.776153	59.234087
2351.382698	84.117183	59.239092
2351.332617	81.271858	59.244097
2351.023761	80.528077	59.249101
2350.339230	89.327806	59.254106
2350.082514	83.234508	59.259111
2348.632440	88.672238	59.264116
2348.260716	91.048835	59.269121
2347.791296	82.477128	59.274125
2346.425906	80.321697	59.279130
2345.923103	84.864448	59.284135
2345.144042	91.895800	59.289140
2344.946412	80.642054	59.294145
2344.636680	83.512112	59.299149
2342.932411	84.515176	59.304154
2342.354212	77.429654	59.309159
2341.591727	83.699906	59.314164
2341.101100	80.032708	59.319169
2340.852940	77.865837	59.324173
2340.329360	95.093800	59.329178
2340.017174	76.389118	59.334183
2338.965593	86.457487	59.339188
2338.117161	85.577823	59.344193
2338.087200	85.343307	59.349197
2336.532153	82.892294	59.354202
2335.787095	77.067630	59.359207
2335.221434	80.378147	59.364212
2334.719337	77.569854	59.369217
2334.376380	79.223531	59.374221
2333.929561	80.579979	59.379226
2333.443678	78.027458	59.384231
2332.585806	85.649765	59.389236
2331.831381	79.927751	59.394241
2330.773831	72.993276	59.399245
2329.976866	79.507047	59.404250
2329.713830	78.328343	59.409255
2329.097065	82.699535	59.414260
2328.282085	74.184162	59.419265
2327.343129	76.393685	59.424269
2326.427592	84.001379	59.429274
2326.478586	75.624890	59.434279
2325.230337	85.988591	59.439284
2324.907109	86.160659	59.444289
2324.707920	80.871051	59.449293
2323.179545	86.994782	59.454298
2322.676671	79.895987	59.459303
2322.006418	91.868031	59.464308
2321.254387	86.881371	59.469313
2320.987713	78.256845	59.474317
2320.197139	92.424387	59.479322
2320.440001	78.881321	59.484327
2319.256623	84.520152	59.489332
2318.388188	87.156945	59.494337
2317.945910	85.176026	59.499341
2316.311049	84.450186	59.504346
2315.819832	83.559966	59.509351
2315.468395	84.975497	59.514356
2314.590180	89.238248	59.519361
2314.487669	82.806359	59.524365
2313.949325	85.045666	59.529370
2313.671410	82.925724	59.534375
2312.303301	90.044385	59.539380
2311.677301	86.353761	59.544385
2311.625331	82.331697	59.549389
2310.829973	80.936927	59.554394
2310.345097	85.380696	59.559399
2309.179760	77.970069	59.564404
2308.312544	78.018457	59.569409
2307.247260	77.079568	59.574413
2306.217256	79.541892	59.579418
2306.203230	75.281244	59.584423
2305.657152	79.544037	59.589428
2305.153583	76.327068	59.594433
2304.538905	75.626508	59.599437
2304.181370	78.448295	59.604442
2303.745946	70.188146	59.609447
2302.266013	77.365397	59.614452
2301.810739	79.807991	59.619457
2301.530273	78.337412	59.624461
2300.219910	81.858958	59.629466
2299.623772	75.878577	59.634471
2298.347328	81.383725	59.639476
2298.007922	75.889949	59.644481
2297.967882	82.585723	59.649485
2297.461144	83.389151	59.654490
2297.243699	73.774142	59.659495
2296.038384	79.864342	59.664500
2295.308746	73.539699	59.669505
2294.928984	78.602574	59.674509
2293.565862	78.369069	59.679514
2292.972876	77.212055	59.684519
2292.098282	86.037970	59.689524
2291.326713	89.265285	59.694529
2291.245260	81.515371	59.699533
2290.596241	82.560228	59.704538
2290.637125	81.867167	59.709543
2289.719285	83.093778	59.714548
2288.564921	83.007727	59.719553
2288.362641	79.783051	59.724557
2287.172414	86.124875	59.729562
2286.418754	76.600378	59.734567
2285.780127	85.438834	59.739572
2285.115173	81.467913	59.744577
2284.791221	76.354377	59.749581
2284.280423	84.903747	59.754586
2283.655349	71.192151	59.759591
2282.130531	87.261104	59.764596
2281.884907	82.260088	59.769601
2281.604332	86.025919	59.774605
2280.969642	85.601142	59.779610
2280.216061	85.478924	59.784615
2279.100462	87.473539	59.789620
2278.730825	88.514436	59.794625
2278.732329	77.105864	59.799629
2277.223844	85.028111	59.804634
2276.264203	82.796603	59.809639
2275.694275	88.055021	59.814644
2275.379141	86.388273	59.819649
2275.250525	85.083562	59.824653
2274.414656	84.084528	59.829658
2273.386849	79.349900	59.834663
2272.714738	86.206655	59.839668
2272.090672	83.268838	59.844673
2271.629916	77.342281	59.849677
2270.371639	80.739272	59.854682
2269.787565	78.350781	59.859687
2268.992954	78.277027	59.864692
2268.572298	82.545215	59.869697
2268.642989	81.194186	59.874701
2267.929543	85.682965	59.879706
2266.746420	84.291752	59.884711
2265.611701	89.107169	59.889716
2265.399255	92.161507	59.894721
2265.459372	87.209257	59.899725
2264.545292	92.327195	59.904730
2263.670468	81.833850	59.909735
2262.902390	89.835530	59.914740
2262.539693	92.245718	59.919745
2262.019742	80.620410	59.924750
2260.998565	99.507223	59.929754
2260.426860	88.231406	59.934759
2259.599284	93.574149	59.939764
2258.050614	78.458975	59.944769
2257.312389	82.528849	59.949774
2257.481118	90.878334	59.954778
2257.377340	73.199842	59.959783
2256.350759	85.961869	59.964788
2256.138300	87.916512	59.969793
2255.180965	86.892464	59.974798
2253.457932	83.244591	59.979802
2253.076428	78.505624	59.984807
2252.503978	79.825538	59.989812
2252.492758	87.535161	59.994817
2251.875130	87.995596	59.999822
2251.243461	83.873335	60.004826
2250.241758	82.175980	60.009831
2249.371143	82.835594	60.014836
2249.089448	79.291357	60.019841
2248.753093	85.928859	60.024846
2247.544311	90.521296	60.029850
2246.504779	82.694843	60.034855
2245.920493	77.901348	60.039860
2245.432480	74.864483	60.044865
2245.400562	76.563257	60.049870
2244.384353	86.514274	60.054874
2244.117342	86.512528	60.059879
2242.754010	90.227086	60.064884
2242.185295	90.556399	60.069889
2241.811715	87.788504	60.074894
2241.365265	89.076215	60.079898
2240.498614	79.494868	60.084903
2239.581397	82.170406	60.089908
2239.000129	82.806986	60.094913
2239.230653	76.215131	60.099918
2237.947589	89.849547	60.104922
2236.883001	78.075816	60.109927
2236.101125	85.747500	60.114932
2235.538384	83.701141	60.119937
2235.585814	84.015871	60.124942
2234.473733	80.993760	60.129946
2233.874333	80.107839	60.134951
2232.778000	69.371745	60.139956
2232.231623	81.294966	60.144961
2232.319469	81.489893	60.149966
2230.775909	76.560857	60.154970
2230.215950	78.835444	60.159975
2229.243643	75.647332	60.164980
2228.942871	80.868404	60.169985
2228.647967	71.363755	60.174990
2228.453261	87.159060	60.179994
2227.649970	74.964874	60.184999
2226.691808	81.328990	60.190004
2226.047963	80.867103	60.195009
2225.544399	67.586703	60.200014
2224.308311	76.812715	60.205018
2223.585804	73.232556	60.210023
2223.054030	78.712993	60.215028
2222.562084	82.372082	60.220033
2222.419379	76.449164	60.225038
2221.087933	82.017414	60.230042
2220.311728	78.761821	60.235047
2219.536506	83.344454	60.240052
2219.011887	83.997005	60.245057
2218.945345	76.400466	60.250062
2218.140852	87.487998	60.255066
2217.149763	72.242757	60.260071
2216.375582	75.834063	60.265076
2215.906954	77.825410	60.270081
2215.483685	76.179529	60.275086
2214.733082	85.150422	60.280090
2213.838394	81.598129	60.285095
2213.075162	78.589783	60.290100
2212.160769	79.050055	60.295105
2211.862217	79.813545	60.300110
2211.503890	83.692537	60.305114
2211.181829	84.576096	60.310119
2210.109246	80.283335	60.315124
2209.519873	82.314279	60.320129
2208.961455	83.726531	60.325134
2208.041100	83.767839	60.330138
2207.191707	78.419316	60.335143
2206.204795	83.922332	60.340148
2205.765547	80.989232	60.345153
2205.716670	80.026532	60.350158
2205.360494	83.742926	60.355162
2204.515839	78.123603	60.360167
2203.491112	76.914519	60.365172
2202.539351	71.332069	60.370177
2202.223202	73.575618	60.375182
2200.919127	79.383522	60.380186
2200.578184	76.241776	60.385191
2199.578827	82.012174	60.390196
2199.158063	76.868233	60.395201
2199.224762	78.122263	60.400206
2198.431039	81.851910	60.405210
2197.888417	74.697570	60.410215
2196.871727	82.761899	60.415220
2195.907275	82.518656	60.420225
2195.940440	75.902530	60.425230
2194.956192	86.211229	60.430234
2193.737362	78.015998	60.435239
2193.223528	78.808807	60.440244
2192.598451	78.203194	60.445249
2192.313003	74.800520	60.450254
2191.667087	74.331098	60.455258
2190.780576	69.900342	60.460263
2190.117439	80.862251	60.465268
2189.227359	76.906166	60.470273
2189.052915	76.079016	60.475278
2188.414791	81.243314	60.480282
2187.733775	68.574301	60.485287
2186.581570	74.339655	60.490292
2186.099944	78.226313	60.495297
2186.207922	72.118034	60.500302
2184.807235	83.382129	60.505306
2183.942273	74.066160	60.510311
2183.184676	77.046762	60.515316
2183.155756	79.647753	60.520321
2182.733110	79.031993	60.525326
2181.671501	83.721239	60.530330
2180.865276	76.275285	60.535335
2179.827061	82.730069	60.540340
2179.119726	80.974884	60.545345
2178.931287	78.594134	60.550350
2178.455615	79.405679	60.555354
2178.220555	84.939976	60.560359
2177.464078	83.260299	60.565364
2176.706079	76.434496	60.570369
2175.936155	77.227685	60.575374
2174.804807	92.989370	60.580378
2174.545538	75.568398	60.585383
2173.789999	88.939710	60.590388
2173.085811	88.283289	60.595393
2172.197552	84.121638	60.600398
2171.140312	89.734973	60.605402
2170.950874	82.316159	60.610407
2170.091569	91.348278	60.615412
2169.838301	89.966209	60.620417
2169.753522	73.806929	60.625422
2168.657175	88.614502	60.630426
2167.981040	86.243742	60.635431
2166.787453	84.067267	60.640436
2166.372488	87.993446	60.645441
2165.774051	84.839295	60.650446
2164.655508	80.237050	60.655450
2164.272987	77.231098	60.660455
2163.778188	85.361694	60.665460
2163.234439	82.091221	60.670465
2162.828793	72.721570	60.675470
2161.426437	79.077191	60.680474
2160.744731	76.757911	60.685479
2160.057467	77.193557	60.690484
2159.631570	81.256599	60.695489
2159.325096	69.840329	60.700494
2159.125223	76.549217	60.705498
2158.154251	73.997973	60.710503
2157.345676	78.206593	60.715508
2156.691854	82.683604	60.720513
2155.736076	71.390225	60.725518
2154.605564	75.613643	60.730522
2153.919471	69.688542	60.735527
2153.969512	77.602008	60.740532
2153.460442	86.733692	60.745537
2153.153700	78.412479	60.750542
2151.694290	83.732638	60.755546
2151.079377	83.896973	60.760551
2150.781233	78.921927	60.765556
2150.366916	76.247850	60.770561
2149.677565	67.748143	60.775566
2148.271458	78.637786	60.780570
2148.030146	81.547855	60.785575
2147.556957	80.901665	60.790580
2146.667311	76.186859	60.795585
2145.772713	73.067577	60.800590
2144.726468	82.014037	60.805594
2144.519332	82.815972	60.810599
2144.288426	79.284373	60.815604
2143.386938	86.702582	60.820609
2142.756058	70.346591	60.825614
2141.740681	85.536220	60.830618
2141.286159	69.918195	60.835623
2140.358028	78.591831	60.840628
2139.803438	81.398381	60.845633
2139.752787	79.584571	60.850638
2138.533984	80.639267	60.855642
2137.794164	73.649319	60.860647
2137.076515	72.446543	60.865652
2136.865910	77.301679	60.870657
2136.476685	76.437453	60.875662
2134.861991	80.493038	60.880666
2134.174100	79.507795	60.885671
2134.043149	83.911564	60.890676
2133.433580	79.145304	60.895681
2133.177746	81.483142	60.900686
2132.478398	88.873886	60.905690
2131.789054	75.440152	60.910695
2131.000715	87.721719	60.915700
2130.387927	77.557794	60.920705
2129.273463	70.737710	60.925710
2128.142389	78.562276	60.930714
2127.613701	72.397107	60.935719
2127.145078	72.363536	60.940724
2126.602059	79.083352	60.945729
2126.752740	72.470027	60.950734
2125.772533	78.167686	60.955738
2125.042391	71.658041	60.960743
2124.451585	73.666737	60.965748
2123.555026	76.999916	60.970753
2122.700388	81.227076	60.975758
2121.755977	77.925273	60.980762
2121.441470	82.338725	60.985767
2120.740795	80.544912	60.990772
2120.483739	81.601297	60.995777
2119.844599	77.230083	61.000782
2118.409539	90.437761	61.005786
2118.231356	80.791981	61.010791
2117.649967	77.962147	61.015796
2116.964043	83.489875	61.020801
2116.589650	75.687062	61.025806
2115.146990	96.802717	61.030810
2114.536678	76.729269	61.035815
2114.033633	79.886991	61.040820
2113.302749	85.345044	61.045825
2113.268389	80.082920	61.050830
2112.644542	86.440395	61.055834
2111.491494	81.047121	61.060839
2110.830544	78.660748	61.065844
2110.367719	84.811477	61.070849
2110.182428	77.359596	61.075854
2108.723726	83.403958	61.080858
2108.120179	85.352865	61.085863
2107.614247	84.891482	61.090868
2107.118083	92.152743	61.095873
2106.397516	85.583040	61.100878
2105.353603	89.380358	61.105882
2104.759469	78.541825	61.110887
2104.136079	85.462883	61.115892
2103.603424	88.082140	61.120897
2103.445552	81.949860	61.125902
2102.672079	85.250544	61.130906
2101.329055	84.034740	61.135911
2100.805687	87.013973	61.140916
2100.245211	88.059101	61.145921
2099.967705	81.502037	61.150926
2099.205096	81.647825	61.155930
2098.188770	75.703035	61.160935
2097.630509	82.880574	61.165940
2097.004204	82.670694	61.170945
2096.816171	74.858903	61.175950
2095.978591	83.233253	61.180954
2095.072911	74.344255	61.185959
2094.253885	81.834017	61.190964
2093.839601	82.781511	61.195969
2093.505817	80.103928	61.200974
2092.229368	76.611432	61.205978
2091.494990	80.361333	61.210983
2091.081446	80.116641	61.215988
2090.488744	87.832554	61.220993
2090.314117	81.669195	61.225998
2088.881904	92.520297	61.231002
2088.456962	81.447571	61.236007
2087.524089	78.418528	61.241012
2087.082987	93.131007	61.246017
2087.105164	78.191688	61.251022
2085.711451	86.635504	61.256026
2084.837964	84.608369	61.261031
2084.476720	81.523393	61.266036
2083.890841	85.086850	61.271041
2083.525955	87.846353	61.276046
2082.403064	82.633448	61.281050
2081.566241	85.419595	61.286055
2081.160353	91.507302	61.291060
2080.841736	85.889209	61.296065
2080.607480	85.365967	61.301070
2079.018106	85.392259	61.306074
2078.127804	84.267573	61.311079
2078.040573	84.851245	61.316084
2077.150589	85.438807	61.321089
2077.145709	86.305224	61.326094
2076.001233	89.555690	61.331098
2075.506187	88.119065	61.336103
2074.601978	82.173652	61.341108
2073.552779	82.904890	61.346113
2072.930218	78.925175	61.351118
2072.010022	73.490113	61.356122
2071.935274	66.341822	61.361127
2071.499918	81.635126	61.366132
2070.863844	80.564058	61.371137
2070.500745	76.848636	61.376142
2069.708895	84.142313	61.381146
2069.046043	85.830983	61.386151
2068.329947	87.124960	61.391156
2066.532198	80.608071	61.396161
2066.487541	79.461501	61.401166
2065.602601	87.715276	61.406170
2065.258909	85.384376	61.411175
2064.748225	76.829255	61.416180
2064.728298	77.898369	61.421185
2063.811971	85.612007	61.426190
2063.041933	89.380248	61.431194
2062.290222	74.291476	61.436199
2060.815076	81.837022	61.441204
2060.185053	85.745518	61.446209
2060.217155	79.737848	61.451214
2059.263222	82.184832	61.456218
2058.872406	81.382461	61.461223
2058.604229	80.868969	61.466228
2057.646465	84.113158	61.471233
2056.820396	73.039190	61.476238
2055.887945	82.889844	61.481242
2055.830664	88.969629	61.486247
2054.818002	80.661811	61.491252
2053.889001	84.086599	61.496257
2053.385518	74.061491	61.501262
2052.881839	75.105591	61.506266
2052.226417	71.213999	61.511271
2051.733238	75.466572	61.516276
2050.261924	75.549255	61.521281
2050.045431	73.517115	61.526286
2049.479305	82.377908	61.531290
2048.767263	76.104382	61.536295
2048.779089	75.629047	61.541300
2047.262867	78.679428	61.546305
2046.729994	70.779005	61.551310
2045.858943	76.428397	61.556314
2045.772731	75.573136	61.561319
2045.592737	73.475939	61.566324
2044.456498	80.406566	61.571329
2043.319677	72.681681	61.576334
2042.615439	78.587925	61.581338
2042.430914	71.133555	61.586343
2041.626130	72.531122	61.591348
2040.375079	79.108770	61.596353
2040.007288	76.923306	61.601358
2039.147872	77.704980	61.606362
2038.864964	69.672989	61.611367
2038.679703	77.105266	61.616372
2038.010452	75.941197	61.621377
2037.298958	75.621953	61.626382
2036.323555	76.766085	61.631386
2035.971461	80.527177	61.636391
2035.055612	81.573100	61.641396
2033.916930	78.049555	61.646401
2033.402882	73.021459	61.651406
2032.676719	78.922375	61.656410
2032.085430	83.475932	61.661415
2032.055347	77.669552	61.666420
2031.418428	77.028091	61.671425
2030.607434	69.768510	61.676430
2029.651041	75.279350	61.681434
2029.264774	76.503492	61.686439
2028.316106	75.906279	61.691444
2027.222046	75.606293	61.696449
2026.618255	71.274443	61.701454
2026.095750	76.983818	61.706458
2025.507933	73.878792	61.711463
2025.071848	80.637160	61.716468
2024.766577	81.178001	61.721473
2024.346999	69.243097	61.726478
2023.084677	81.008919	61.731482
2022.256431	68.444474	61.736487
2022.110442	77.530230	61.741492
2020.979006	70.677161	61.746497
2020.435483	66.555259	61.751502
2019.603927	74.247289	61.756506
2019.268194	65.410030	61.761511
2018.848531	69.332277	61.766516
2017.861410	72.423602	61.771521
2017.179351	70.131641	61.776526
2016.255901	74.413211	61.781530
2016.000611	68.959162	61.786535
2015.309960	64.957555	61.791540
2013.936422	70.272524	61.796545
2013.976196	61.050522	61.801550
2013.087372	65.439453	61.806554
2012.734820	66.557569	61.811559
2012.367298	64.126546	61.816564
2010.891191	67.079682	61.821569
2010.328468	67.317997	61.826574
2009.788529	71.253319	61.831578
2009.391164	66.682486	61.836583
2009.156508	68.033847	61.841588
2007.613823	64.540737	61.846593
2007.124121	60.139248	61.851598
2006.623788	71.684331	61.856602
2006.035929	69.707823	61.861607
2005.051905	64.646052	61.866612
2004.157781	67.493322	61.871617
2003.778878	54.722956	61.876622
2003.227450	74.719069	61.881626
2002.871252	66.896983	61.886631
2002.605728	71.471784	61.891636
2000.821336	72.792594	61.896641
2000.327085	68.750683	61.901646
1999.739031	68.962149	61.906650
1999.365664	74.130507	61.911655
1999.186544	77.576628	61.916660
1998.072752	70.349904	61.921665
1997.483809	71.109000	61.926670
1996.897192	77.007757	61.931674
1996.206354	72.021355	61.936679
1995.183937	66.432490	61.941684
1994.617501	73.016187	61.946689
1994.073275	61.980478	61.951694
1993.611855	70.883747	61.956698
1993.113943	71.852657	61.961703
1991.946927	67.522031	61.966708
1991.085662	65.689791	61.971713
1990.596423	63.565765	61.976718
1990.493614	71.704693	61.981722
1989.814880	66.548466	61.986727
1988.921989	75.166349	61.991732
1988.028693	76.228157	61.996737
1987.856671	64.887997	62.001742
1986.510158	68.092512	62.006746
1985.456127	74.540548	62.011751
1985.345934	70.880556	62.016756
1984.844142	69.098136	62.021761
1984.222311	64.053358	62.026766
1983.721072	71.152459	62.031770
1982.598527	71.417859	62.036775
1981.727759	66.400269	62.041780
1981.079435	78.603409	62.046785
1980.964674	65.595231	62.051790
1980.663650	75.028016	62.056794
1979.798214	67.127656	62.061799
1978.940008	71.673190	62.066804
1978.185930	62.467783	62.071809
1977.726174	61.218152	62.076814
1976.671836	65.858023	62.081818
1975.603907	66.166579	62.086823
1975.563856	72.159331	62.091828
1974.356124	65.493796	62.096833
1974.090045	62.226774	62.101838
1973.702740	71.751286	62.106842
1973.230271	64.200927	62.111847
1972.230825	62.125498	62.116852
1971.418911	73.484285	62.121857
1971.168246	62.169424	62.126862
1970.521250	71.118254	62.131866
1969.854938	66.516463	62.136871
1969.036546	68.926063	62.141876
1967.894886	73.759288	62.146881
1967.767075	63.296535	62.151886
1967.095213	67.037329	62.156890
1966.289906	68.662749	62.161895
1965.707775	72.526347	62.166900
1965.105674	74.028589	62.171905
1964.611287	67.260764	62.176910
1963.198086	73.572489	62.181914
1962.754069	71.519672	62.186919
1962.192748	67.586737	62.191924
1962.008117	73.364625	62.196929
1961.605521	72.099297	62.201934
1960.398249	68.190022	62.206938
1959.472015	66.182594	62.211943
1959.390109	71.814625	62.216948
1958.419407	76.969515	62.221953
1957.846603	62.933296	62.226958
1956.918696	73.273415	62.231962
1956.523127	63.481705	62.236967
1955.996573	59.915836	62.241972
1954.662114	67.622848	62.246977
1953.660999	66.688450	62.251982
1953.198384	68.970088	62.256986
1952.752148	65.459160	62.261991
1952.661051	67.295154	62.266996
1951.899741	70.906784	62.272001
1951.642738	59.117374	62.277006
1950.423330	70.942563	62.282010
1949.480919	62.439617	62.287015
1948.750389	65.248250	62.292020
1948.311750	64.729980	62.297025
1947.998668	69.362257	62.302030
1947.539821	63.447664	62.307034
1946.700792	67.001934	62.312039
1946.031796	68.132742	62.317044
1945.385372	62.747586	62.322049
1944.600833	57.328430	62.327054
1943.406601	74.054113	62.332058
1942.487724	78.994885	62.337063
1942.406849	73.929014	62.342068
1941.602563	69.392276	62.347073
1941.452466	69.090687	62.352078
1941.252934	77.000645	62.357082
1939.850948	73.142052	62.362087
1939.360491	68.695701	62.367092
1938.444470	70.634132	62.372097
1938.164160	68.044123	62.377102
1936.700401	70.408215	62.382106
1936.045948	73.596190	62.387111
1935.880904	66.489015	62.392116
1935.043853	75.298656	62.397121
1934.800757	65.621781	62.402126
1934.554540	75.402805	62.407130
1933.496666	64.157357	62.412135
1932.799794	70.689951	62.417140
1931.815333	74.886842	62.422145
1931.505909	58.235155	62.427150
1930.207199	65.534623	62.432154
1929.557705	66.746172	62.437159
1929.133008	67.347709	62.442164
1928.712629	64.402337	62.447169
1928.179687	68.772238	62.452174
1927.543202	71.648468	62.457178
1926.534668	69.387109	62.462183
1925.916878	67.576384	62.467188
1925.333104	73.309664	62.472193
1925.019961	61.013962	62.477198
1923.559553	68.652529	62.482202
1923.082940	67.736563	62.487207
1922.780065	67.729522	62.492212
1922.035288	62.822229	62.497217
1921.920217	60.783010	62.502222
1920.917264	65.082139	62.507226
1919.876921	68.502701	62.512231
1919.533264	67.901082	62.517236
1918.628445	73.487581	62.522241
1918.400307	64.727454	62.527246
1917.357232	70.771403	62.532250
1916.463198	66.506198	62.537255
1915.995482	66.217107	62.542260
1915.504625	69.917073	62.547265
1915.491509	67.000315	62.552270
1914.185380	62.970209	62.557274
1913.225592	66.830920	62.562279
1913.149054	63.467137	62.567284
1911.509148	67.345914	62.572289
1911.293362	69.583749	62.577294
1910.334843	72.759404	62.582298
1909.759924	71.054632	62.587303
1909.629381	67.706798	62.592308
1908.971668	72.900908	62.597313
1908.545328	61.658742	62.602318
1907.641193	67.259333	62.607322
1906.678151	70.923242	62.612327
1906.581918	64.632029	62.617332
1905.486601	69.090245	62.622337
1905.077063	63.556023	62.627342
1904.072095	63.357264	62.632346
1903.708540	65.919971	62.637351
1903.025212	59.461577	62.642356
1902.277667	59.596922	62.647361
1901.299017	61.299371	62.652366
1900.315052	62.404334	62.657370
1899.907332	66.188758	62.662375
1899.699568	57.668694	62.667380
1899.109804	68.876980	62.672385
1898.704485	61.664870	62.677390
1897.571748	59.774490	62.682394
1896.755348	67.491563	62.687399
1896.534714	66.985737	62.692404
1895.745503	73.407031	62.697409
1895.341589	63.753333	62.702414
1894.214901	67.050124	62.707418
1893.910682	69.635838	62.712423
1893.808336	68.975964	62.717428
1892.068404	74.083652	62.722433
1891.252859	60.880394	62.727438
1891.157883	60.950283	62.732442
1890.527593	65.958129	62.737447
1889.465960	65.238168	62.742452
1888.134018	66.204120	62.747457
1888.570669	59.065460	62.752462
1887.416294	66.103411	62.757466
1887.278496	63.577444	62.762471
1886.887050	60.225303	62.767476
1885.496217	66.057575	62.772481
1884.735160	69.375892	62.777486
1883.999590	63.694169	62.782490
1883.492822	65.574039	62.787495
1883.721411	66.123023	62.792500
1882.782740	62.012300	62.797505
1881.708013	65.664135	62.802510
1880.973672	69.142480	62.807514
1880.675457	69.701857	62.812519
1880.086452	66.580478	62.817524
1878.922707	70.337146	62.822529
1878.166990	62.530539	62.827534
1877.939797	64.794403	62.832538
1877.145339	61.321350	62.837543
1876.663654	56.051309	62.842548
1875.340225	69.986317	62.847553
1874.921193	68.015286	62.852558
1874.286340	75.730515	62.857562
1873.904249	72.888724	62.862567
1873.938484	64.011483	62.867572
1872.716579	62.135968	62.872577
1871.932671	62.694757	62.877582
1871.197994	70.988750	62.882586
1870.642695	63.606126	62.887591
1869.640892	62.169779	62.892596
1868.753830	70.704964	62.897601
1868.542301	69.236436	62.902606
1868.122847	73.307858	62.907610
1867.257370	64.601120	62.912615
1867.329905	65.570338	62.917620
1865.838496	72.720822	62.922625
1865.097387	67.658576	62.927630
1864.693763	66.768022	62.932634
1863.719375	77.681737	62.937639
1862.957459	62.533207	62.942644
1862.187942	78.887828	62.947649
1861.906519	74.842285	62.952654
1861.693201	63.151595	62.957658
1860.810602	74.690630	62.962663
1859.941437	68.954006	62.967668
1858.985732	75.624042	62.972673
1858.307565	80.000244	62.977678
1858.024747	78.684038	62.982682
1857.668635	71.559823	62.987687
1857.160655	64.300942	62.992692
1855.844884	79.581831	62.997697
1855.423246	73.617464	63.002702
1854.849852	76.693292	63.007706
1853.593810	78.231639	63.012711
1852.605708	71.019373	63.017716
1852.349782	73.948128	63.022721
1851.733117	66.153654	63.027726
1851.132186	73.839396	63.032730
1850.985230	71.760636	63.037735
1851.002076	66.128605	63.042740
1849.761040	74.536466	63.047745
1848.863770	64.381418	63.052750
1848.523039	74.467146	63.057754
1847.136198	69.263153	63.062759
1846.381767	70.623711	63.067764
1845.467545	72.789602	63.072769
1845.343618	67.899652	63.077774
1844.952921	76.893055	63.082778
1844.499997	61.985734	63.087783
1843.558387	64.001974	63.092788
1842.582702	71.221722	63.097793
1842.144252	62.220100	63.102798
1841.503513	62.599669	63.107802
1840.836785	64.382178	63.112807
1839.951315	70.143789	63.117812
1839.099496	68.971906	63.122817
1838.536030	67.800425	63.127822
1838.441334	67.728562	63.132826
1837.845632	67.919249	63.137831
1837.074515	67.277090	63.142836
1836.108155	74.210651	63.147841
1835.494071	66.066411	63.152846
1834.955468	63.963479	63.157850
1834.653976	62.117599	63.162855
1833.691973	62.751073	63.167860
1832.433648	65.496473	63.172865
1832.304016	65.665840	63.177870
1831.532586	66.745110	63.182874
1830.827783	71.953992	63.187879
1830.333417	64.118469	63.192884
1829.472609	74.327122	63.197889
1829.220590	71.951746	63.202894
1828.253871	70.632952	63.207898
1826.993271	72.554567	63.212903
1826.613479	63.545280	63.217908
1825.729818	66.061982	63.222913
1825.610972	65.788602	63.227918
1825.202884	68.191966	63.232922
1824.720708	69.775146	63.237927
1823.767140	77.846079	63.242932
1822.654080	83.187969	63.247937
1822.405261	67.565624	63.252942
1822.275135	72.133444	63.257946
1820.970533	69.241870	63.262951
1820.360699	65.087924	63.267956
1819.003365	71.706289	63.272961
1818.784694	71.762606	63.277966
1818.701761	67.754554	63.282970
1818.087865	75.912233	63.287975
1816.797988	60.824840	63.292980
1816.284975	80.126763	63.297985
1815.478399	69.207814	63.302990
1815.182033	65.909672	63.307994
1814.402264	64.851382	63.312999
1813.905358	62.951310	63.318004
1812.930662	66.681959	63.323009
1812.789484	65.197057	63.328014
1811.947440	73.342061	63.333018
1810.755799	72.610414	63.338023
1810.504828	61.043013	63.343028
1809.653562	68.375681	63.348033
1809.420356	72.758251	63.353038
1808.726618	70.467530	63.358042
1807.794697	76.192490	63.363047
1807.218985	71.113798	63.368052
1806.375165	65.245751	63.373057
1805.649862	60.935914	63.378062
1804.579354	68.368854	63.383066
1804.127095	69.467726	63.388071
1803.561729	67.007023	63.393076
1803.116899	67.610436	63.398081
1802.736756	62.160800	63.403086
1802.319902	58.794069	63.408090
1801.118982	63.561672	63.413095
1800.791199	60.063653	63.418100
1800.048792	58.451893	63.423105
1799.408639	61.721505	63.428110
1798.309636	69.962972	63.433114
1797.530059	69.204244	63.438119
1796.961983	65.180125	63.443124
1796.706518	70.194503	63.448129
1796.291517	70.187311	63.453134
1795.072878	66.681457	63.458138
1794.137206	71.522097	63.463143
1793.773241	68.194471	63.468148
1793.193200	67.394895	63.473153
1793.261824	65.307278	63.478158
1792.075585	67.247361	63.483162
1791.208808	67.518775	63.488167
1790.632610	59.654238	63.493172
1790.100218	67.948752	63.498177
1789.578874	63.791512	63.503182
1788.776918	61.049596	63.508186
1787.640306	66.203287	63.513191
1787.393751	54.502514	63.518196
1786.636901	62.076777	63.523201
1785.834211	68.513411	63.528206
1785.137638	68.022314	63.533210
1784.753928	72.560497	63.538215
1784.215889	64.245765	63.543220
1783.753951	73.938957	63.548225
1782.614201	67.152904	63.553230
1782.063473	68.410726	63.558234
1781.363942	70.361085	63.563239
1781.176899	62.227078	63.568244
1779.521242	69.929475	63.573249
1779.221101	63.827496	63.578254
1778.919763	71.021077	63.583258
1778.115656	69.223305	63.588263
1777.882208	58.182628	63.593268
1776.480654	63.492173	63.598273
1776.051822	68.985010	63.603278
1775.715407	70.829031	63.608282
1774.615037	63.480874	63.613287
1773.554371	62.819585	63.618292
1772.843871	60.777256	63.623297
1772.506663	69.087714	63.628302
1772.166394	70.070327	63.633306
1771.458535	78.994054	63.638311
1771.356494	68.109302	63.643316
1770.508151	70.513789	63.648321
1769.770208	70.326602	63.653326
1769.222829	72.711567	63.658330
1768.100475	70.712865	63.663335
1767.306472	60.267027	63.668340
1766.361590	73.165874	63.673345
1765.988605	72.389291	63.678350
1765.716299	74.399968	63.683354
1764.760115	76.094651	63.688359
1764.762410	71.031930	63.693364
1763.348811	78.327407	63.698369
1762.759284	59.054589	63.703374
1762.466910	66.493333	63.708378
1761.304160	71.709921	63.713383
1761.042936	68.745230	63.718388
1760.121701	76.913263	63.723393
1759.789853	79.320560	63.728398
1759.188990	74.207890	63.733402
1757.731411	76.848459	63.738407
1756.807434	64.494283	63.743412
1756.577588	70.554626	63.748417
1756.092656	69.426162	63.753422
1755.685688	66.683375	63.758426
1754.840358	78.214855	63.763431
1754.845353	56.487786	63.768436
1753.804695	71.082551	63.773441
1752.941709	71.092807	63.778446
1752.658432	66.631165	63.783450
1751.604864	72.343788	63.788455
1750.559450	71.127681	63.793460
1750.142901	73.985241	63.798465
1749.494201	69.441261	63.803470
1749.178746	62.482208	63.808474
1748.434797	67.156237	63.813479
1748.476216	63.818067	63.818484
1747.122877	65.820696	63.823489
1746.505067	66.033729	63.828494
1745.944245	67.787470	63.833498
1744.854024	70.435050	63.838503
1743.993107	66.282632	63.843508
1743.220954	75.359064	63.848513
1743.003040	77.029660	63.853518
1742.412990	75.587224	63.858522
1741.952237	71.027270	63.863527
1741.557547	73.295721	63.868532
1740.610712	69.745347	63.873537
1740.280860	75.122965	63.878542
1738.923957	67.780028	63.883546
1738.130069	72.628781	63.888551
1737.429397	62.976156	63.893556
1736.435838	80.166837	63.898561
1736.511185	68.872410	63.903566
1736.099080	66.096952	63.908570
1735.162609	74.089969	63.913575
1734.176546	63.852651	63.918580
1733.450222	74.130267	63.923585
1733.103384	64.921944	63.928590
1732.859283	68.129323	63.933594
1731.879561	80.963484	63.938599
1730.920480	64.433263	63.943604
1730.133216	72.919016	63.948609
1729.689742	66.073839	63.953614
1729.464036	73.552492	63.958618
1728.912243	72.336001	63.963623
1727.765691	66.463722	63.968628
1726.960300	71.997705	63.973633
1726.351972	68.575721	63.978638
1726.072715	71.787931	63.983642
1725.604988	72.075544	63.988647
1724.566285	64.631984	63.993652
1723.496654	73.822078	63.998657
1723.062597	71.487727	64.003662
1723.117505	68.277901	64.008666
1721.929397	72.876362	64.013671
1721.036411	66.788599	64.018676
1720.144261	66.795956	64.023681
1719.849151	68.981844	64.028686
1719.511680	69.710966	64.033690
1719.090191	79.593019	64.038695
1718.036989	65.716427	64.043700
1717.375993	65.140308	64.048705
1716.476495	59.371807	64.053710
1716.469792	66.447077	64.058714
1715.160532	71.253761	64.063719
1714.648802	70.714862	64.068724
1713.974795	66.508364	64.073729
1713.599549	64.426045	64.078734
1712.674506	60.205270	64.083738
1711.790398	70.076481	64.088743
1711.146926	59.756078	64.093748
1710.734174	68.149721	64.098753
1709.951273	67.365130	64.103758
1709.848919	57.251335	64.108762
1708.520815	65.742397	64.113767
1707.968815	64.732383	64.118772
1707.396565	70.033851	64.123777
1706.775766	63.334279	64.128782
1706.269193	65.485302	64.133786
1704.580730	65.376695	64.138791
1704.548084	65.522365	64.143796
1704.133035	70.144067	64.148801
1703.851793	64.692914	64.153806
1703.264083	56.942861	64.158810
1701.936904	68.589550	64.163815
1701.469798	63.986482	64.168820
1700.969724	59.059861	64.173825
1700.097856	56.936214	64.178830
1699.215016	60.894702	64.183834
1698.120136	63.457827	64.188839
1698.325502	51.159107	64.193844
1697.822188	56.246678	64.198849
1697.461631	64.855588	64.203854
1696.447032	60.493437	64.208858
1695.795506	67.589049	64.213863
1694.744545	62.644593	64.218868
1693.440985	71.816694	64.223873
1692.926541	69.538731	64.228878
1693.138165	70.946756	64.233882
1691.860363	74.006559	64.238887
1691.676481	67.042365	64.243892
1691.116221	70.580148	64.248897
1690.421734	66.698855	64.253902
1689.604079	65.801404	64.258906
1688.537486	73.237242	64.263911
1688.359194	64.923335	64.268916
1687.541711	72.103398	64.273921
1687.149108	66.817743	64.278926
1686.061600	61.309174	64.283930
1685.168631	69.076469	64.288935
1684.828275	61.783805	64.293940
1684.454824	62.405801	64.298945
1683.836626	65.379180	64.303950
1682.979293	57.560010	64.308954
1682.432037	64.024779	64.313959
1681.872475	64.325348	64.318964
1681.144108	63.415777	64.323969
1679.838565	64.786192	64.328974
1679.118198	68.780038	64.333978
1678.338777	70.644215	64.338983
1678.298626	67.741960	64.343988
1677.800069	69.584127	64.348993
1677.512358	73.267897	64.353998
1676.821772	67.432865	64.359002
1675.588775	72.644121	64.364007
1675.317664	63.386536	64.369012
1674.706023	67.664921	64.374017
1673.524054	67.876216	64.379022
1672.553703	66.983187	64.384026
1672.168733	67.718860	64.389031
1672.026057	66.725646	64.394036
1671.539379	71.324476	64.399041
1670.294426	71.468394	64.404046
1669.778742	69.429847	64.409050
1668.840507	71.143972	64.414055
1668.589731	69.600465	64.419060
1667.951454	67.114364	64.424065
1666.533030	65.052277	64.429070
1666.073021	64.056131	64.434074
1666.160027	68.476663	64.439079
1665.927139	62.341876	64.444084
1664.622424	65.851533	64.449089
1663.915390	67.715166	64.454094
1663.197039	63.496135	64.459098
1662.410701	67.295227	64.464103
1661.733703	64.675628	64.469108
1660.748057	67.898197	64.474113
1659.803129	75.700835	64.479118
1659.761909	66.746922	64.484122
1659.313535	66.653877	64.489127
1658.746872	62.060353	64.494132
1658.349535	67.475174	64.499137
1657.215136	66.841921	64.504142
1656.694820	72.080428	64.509146
1655.783323	72.212680	64.514151
1654.979658	60.289117	64.519156
1653.603343	60.921681	64.524161
1653.315067	62.044212	64.529166
1652.944672	59.383201	64.534170
1652.340171	61.722688	64.539175
1652.549601	57.132536	64.544180
1651.807473	67.307465	64.549185
1650.945584	66.173259	64.554190
1650.316428	60.221938	64.559194
1649.370466	73.308466	64.564199
1649.093559	62.306033	64.569204
1647.680692	68.426718	64.574209
1647.014669	70.957121	64.579214
1646.837370	67.947290	64.584218
1645.835667	62.446152	64.589223
1645.078331	65.240459	64.594228
1644.336053	65.507565	64.599233
1643.925729	67.212272	64.604238
1643.550852	64.786097	64.609242
1642.806460	65.920762	64.614247
1642.307919	66.368386	64.619252
1641.166442	69.477499	64.624257
1640.703156	72.491871	64.629262
1640.029284	66.548991	64.634266
1639.177404	72.917086	64.639271
1638.742285	63.886116	64.644276
1637.821361	70.740083	64.649281
1637.035404	75.859452	64.654286
1636.802900	69.079629	64.659290
1636.131036	73.853040	64.664295
1635.871854	71.355752	64.669300
1634.922218	65.030610	64.674305
1634.306012	76.306183	64.679310
1634.066338	71.062256	64.684314
1632.620166	71.074440	64.689319
1632.148640	64.910628	64.694324
1631.350979	66.509918	64.699329
1630.551813	62.375773	64.704334
1629.499797	64.216344	64.709338
1628.998313	67.641050	64.714343
1628.839256	59.743449	64.719348
1627.782978	66.702679	64.724353
1627.314764	67.012488	64.729358
1627.257720	64.070103	64.734362
1626.470783	64.137625	64.739367
1625.638474	70.742361	64.744372
1624.785947	69.503140	64.749377
1623.891994	63.310571	64.754382
1623.720885	56.348151	64.759386
1622.631816	65.526183	64.764391
1621.887945	61.273240	64.769396
1621.306949	69.036098	64.774401
1620.832987	69.535962	64.779406
1620.520741	63.484626	64.784410
1619.791108	71.201477	64.789415
1619.112041	65.429615	64.794420
1617.957679	60.869174	64.799425
1617.449638	64.862609	64.804430
1617.134873	66.635435	64.809434
1616.137131	68.001742	64.814439
1615.187871	65.339930	64.819444
1614.506320	68.608751	64.824449
1614.441531	67.792859	64.829454
1614.265321	65.159406	64.834458
1612.847743	69.124948	64.839463
1611.637866	67.418749	64.844468
1611.341255	66.282151	64.849473
1610.804403	70.267493	64.854478
1610.848036	69.751585	64.859482
1610.126313	71.842334	64.864487
1609.163220	66.131711	64.869492
1608.186620	60.211437	64.874497
1607.507552	65.108838	64.879502
1607.412403	61.903776	64.884506
1606.357832	73.025034	64.889511
1605.664823	62.115921	64.894516
1605.049018	61.821018	64.899521
1604.726197	70.944501	64.904526
1603.740297	60.063015	64.909530
1602.837280	69.797738	64.914535
1602.498826	67.812944	64.919540
1602.140692	61.392902	64.924545
1601.220216	59.561000	64.929550
1600.426674	63.503036	64.934554
1599.872975	60.464865	64.939559
1598.977539	62.880197	64.944564
1597.783895	61.801591	64.949569
1597.002381	66.243652	64.954574
1597.307651	61.356848	64.959578
1596.284188	64.330908	64.964583
1595.966668	64.455860	64.969588
1595.171601	63.086817	64.974593
1594.657542	65.065058	64.979598
1593.737744	60.605396	64.984602
1592.699319	69.981205	64.989607
1592.551511	64.920501	64.994612
1591.976989	61.073168	64.999617
1591.387286	63.064749	65.004622
1590.256952	62.206616	65.009626
1589.364785	66.930102	65.014631
1588.976692	68.963757	65.019636
1588.805718	70.310153	65.024641
1588.339342	66.389446	65.029646
1587.644144	59.645791	65.034650
1586.515718	70.007617	65.039655
1586.388187	58.104147	65.044660
1585.044208	69.081125	65.049665
1584.048978	67.205574	65.054670
1583.428941	64.547030	65.059674
1582.756867	62.418027	65.064679
1582.837045	59.371243	65.069684
1582.455548	59.831602	65.074689
1581.093161	57.142216	65.079694
1580.468732	67.412263	65.084698
1579.741487	63.833030	65.089703
1579.461953	60.446377	65.094708
1578.977467	60.959492	65.099713
1578.013433	62.372534	65.104718
1577.297304	55.798642	65.109722
1576.676134	66.685076	65.114727
1576.171172	57.440295	65.119732
1574.988922	61.049795	65.124737
1574.251005	69.754863	65.129742
1574.277520	58.811829	65.134746
1573.281938	61.940983	65.139751
1573.074327	60.640348	65.144756
1571.675670	65.716557	65.149761
1570.430053	65.785222	65.154766
1570.031791	62.950179	65.159770
1569.552138	69.202078	65.164775
1569.506786	58.225163	65.169780
1569.258914	59.978253	65.174785
1568.571541	68.708617	65.179790
1567.844480	59.732362	65.184794
1566.827221	72.677154	65.189799
1566.344922	66.392043	65.194804
1564.899228	73.025973	65.199809
1564.021379	65.731764	65.204814
1563.915484	56.245803	65.209818
1563.317074	67.183208	65.214823
1562.848819	65.035904	65.219828
1562.446006	65.466757	65.224833
1561.565057	66.601910	65.229838
1560.735395	55.541735	65.234842
1560.368897	71.469750	65.239847
1559.292874	57.929480	65.244852
1558.510436	66.642957	65.249857
1557.519418	64.437889	65.254862
1557.091398	60.433653	65.259866
1556.300598	68.180711	65.264871
1556.332033	57.028821	65.269876
1556.082334	64.040275	65.274881
1555.295009	67.295625	65.279886
1554.890448	67.835721	65.284890
1553.642471	71.752120	65.289895
1552.515288	64.894515	65.294900
1552.341856	67.895994	65.299905
1550.789206	70.252110	65.304910
1550.689468	64.978323	65.309914
1550.031375	69.085860	65.314919
1549.883381	59.311854	65.319924
1549.758340	59.908317	65.324929
1548.389961	63.958212	65.329934
1548.061004	61.223806	65.334938
1546.227253	66.987088	65.339943
1545.494407	54.331078	65.344948
1545.158373	60.488924	65.349953
1544.377165	64.379516	65.354958
1544.593797	60.868478	65.359962
1543.909446	66.108220	65.364967
1543.386626	65.221516	65.369972
1542.426282	64.839146	65.374977
1541.473937	69.242953	65.379982
1541.122008	54.593155	65.384986
1540.410377	67.467480	65.389991
1539.533100	64.611401	65.394996
1538.774856	71.520822	65.400001
1538.223025	64.519360	65.405006
1537.776091	61.297933	65.410010
1537.053158	73.226083	65.415015
1536.323150	68.904074	65.420020
1535.541697	66.671039	65.425025
1534.709371	63.730692	65.430030
1534.562633	66.983380	65.435034
1533.866898	71.045258	65.440039
1532.777576	65.615588	65.445044
1532.220359	64.794375	65.450049
1531.734353	68.554712	65.455054
1531.815968	63.711711	65.460058
1530.645748	61.969537	65.465063
1529.938286	56.575960	65.470068
1529.583920	61.419373	65.475073
1527.933444	51.268208	65.480078
1526.672979	57.736628	65.485082
1526.368652	64.328372	65.490087
1526.661349	62.781856	65.495092
1526.235864	62.778849	65.500097
1525.224889	57.773913	65.505102
1524.879597	54.243001	65.510106
1523.392097	62.963073	65.515111
1522.647678	62.934129	65.520116
1522.182705	65.712359	65.525121
1521.759275	64.398139	65.530126
1521.598266	56.412074	65.535130
1520.497043	67.087393	65.540135
1519.378177	56.838532	65.545140
1519.003825	64.024075	65.550145
1518.568241	69.638857	65.555150
1518.368659	57.115785	65.560154
1517.345832	63.178818	65.565159
1516.381760	57.960603	65.570164
1515.889911	64.500760	65.575169
1515.225893	66.044036	65.580174
1514.622973	57.433768	65.585178
1513.478127	66.931608	65.590183
1512.617211	61.526008	65.595188
1512.041598	59.256565	65.600193
1511.449302	71.992054	65.605198
1511.324641	61.616059	65.610202
1511.107234	70.661105	65.615207
1510.381672	66.088878	65.620212
1509.361694	68.830658	65.625217
1508.970888	65.588969	65.630222
1508.527665	57.923562	65.635226
1507.175964	61.873905	65.640231
1506.310990	61.449957	65.645236
1506.251518	66.473416	65.650241
1505.309602	73.558744	65.655246
1504.652395	63.346128	65.660250
1503.759686	68.900207	65.665255
1503.229209	59.357452	65.670260
1502.987067	58.971767	65.675265
1502.034170	67.084450	65.680270
1501.076843	67.555744	65.685274
1500.165317	74.234047	65.690279
1500.186838	67.404447	65.695284
1499.656291	60.921959	65.700289
1498.476164	77.871031	65.705294
1497.806120	68.575175	65.710298
1497.170882	71.210451	65.715303
1496.451722	68.890581	65.720308
1496.364789	66.455003	65.725313
1495.577896	73.023163	65.730318
1495.202430	66.285194	65.735322
1493.848395	69.490317	65.740327
1493.409425	71.473477	65.745332
1492.994931	72.129746	65.750337
1492.075245	67.524434	65.755342
1491.474305	65.325641	65.760346
1490.916069	69.022557	65.765351
1490.449227	67.296185	65.770356
1489.132171	60.939629	65.775361
1488.338518	74.073513	65.780366
1487.877784	66.190060	65.785370
1487.184800	72.060468	65.790375
1486.451169	74.750085	65.795380
1486.599165	67.062826	65.800385
1485.585519	74.399237	65.805390
1484.628116	63.032536	65.810394
1483.647592	64.352500	65.815399
1483.574204	69.641618	65.820404
1483.285422	68.125943	65.825409
1482.221112	69.529324	65.830414
1481.853627	72.165746	65.835418
1481.262075	62.191362	65.840423
1480.230038	67.998227	65.845428
1479.398263	58.766377	65.850433
1478.479305	66.034081	65.855438
1478.173903	60.758794	65.860442
1477.814499	61.890743	65.865447
1477.555491	64.576094	65.870452
1476.156128	66.014719	65.875457
1475.388084	71.093932	65.880462
1475.026653	59.427083	65.885466
1473.809537	72.082417	65.890471
1473.065449	72.501034	65.895476
1472.295876	71.294219	65.900481
1471.843602	72.088792	65.905486
1471.153257	60.055100	65.910490
1470.756816	65.278331	65.915495
1470.291706	61.165591	65.920500
1469.938161	64.473411	65.925505
1469.391821	68.474594	65.930510
1468.395358	66.988471	65.935514
1467.308572	66.889456	65.940519
1467.301424	69.106982	65.945524
1467.109751	59.541375	65.950529
1465.572447	69.042845	65.955534
1464.945799	58.942638	65.960538
1464.273738	68.888881	65.965543
1463.864445	62.360777	65.970548
1462.915719	65.730997	65.975553
1461.656267	68.904544	65.980558
1461.787782	67.728624	65.985562
1461.192965	66.007975	65.990567
1460.401445	61.807822	65.995572
1459.630118	71.502254	66.000577
1458.626427	77.379270	66.005582
1458.596293	68.385587	66.010586
1457.812535	75.503847	66.015591
1457.492107	68.044389	66.020596
1456.696565	69.421509	66.025601
1455.614082	71.812039	66.030606
1455.228585	69.418487	66.035610
1454.356698	67.983278	66.040615
1453.531467	67.035456	66.045620
1452.975777	65.192458	66.050625
1452.167116	75.040118	66.055630
1451.713004	61.616058	66.060634
1451.330363	71.450794	66.065639
1450.883061	69.606612	66.070644
1449.867237	65.511165	66.075649
1449.081061	69.506824	66.080654
1448.697356	65.210818	66.085658
1447.791940	66.056507	66.090663
1446.733848	72.797005	66.095668
1446.335882	61.507448	66.100673
1445.749610	71.339145	66.105678
1445.458129	61.840358	66.110682
1444.997958	70.920242	66.115687
1444.055796	66.283265	66.120692
1443.112208	65.185184	66.125697
1442.661982	67.343555	66.130702
1441.802556	69.185538	66.135706
1440.719059	65.042468	66.140711
1440.104347	65.217903	66.145716
1439.776806	63.982010	66.150721
1439.238548	70.509195	66.155726
1438.972929	63.022994	66.160730
1438.006328	63.068405	66.165735
1437.036874	61.209395	66.170740
1436.709124	68.329728	66.175745
1435.720284	63.941127	66.180750
1435.258912	56.136741	66.185754
1434.777698	65.220618	66.190759
1434.011627	62.098037	66.195764
1433.511440	58.578253	66.200769
1432.459911	67.304245	66.205774
1432.045164	60.986676	66.210778
1430.886029	62.954955	66.215783
1430.314805	68.810840	66.220788
1429.873065	61.074142	66.225793
1429.393678	67.240345	66.230798
1429.136259	75.196893	66.235802
1427.933457	80.298427	66.240807
1427.134084	74.669555	66.245812
1426.967406	58.019214	66.250817
1426.175502	68.259511	66.255822
1425.569796	59.342646	66.260826
1424.600834	68.359229	66.265831
1423.748727	63.203972	66.270836
1423.634035	60.850910	66.275841
1422.677452	72.665903	66.280846
1422.039378	70.760040	66.285850
1421.108840	74.078999	66.290855
1420.322489	68.972087	66.295860
1420.090769	61.636395	66.300865
1419.465310	60.222957	66.305870
1419.519870	56.045352	66.310874
1418.457097	67.170788	66.315879
1417.681859	69.697410	66.320884
1416.948278	65.143942	66.325889
1415.592366	67.837849	66.330894
1414.896639	61.984411	66.335898
1414.259788	66.800394	66.340903
1413.975132	66.029246	66.345908
1413.669888	54.293587	66.350913
1412.882625	63.439717	66.355918
1412.576024	55.125314	66.360922
1411.331104	64.332020	66.365927
1410.732300	60.004157	66.370932
1410.782198	55.391582	66.375937
1409.503904	65.884861	66.380942
1408.493763	63.607314	66.385946
1407.755199	66.509352	66.390951
1407.274840	63.813506	66.395956
1407.003039	63.978798	66.400961
1406.658352	75.374070	66.405966
1406.143347	62.250167	66.410970
1405.184218	60.042833	66.415975
1404.431382	63.242958	66.420980
1403.402481	61.248084	66.425985
1402.574811	65.064543	66.430990
1401.931203	55.752745	66.435994
1401.214043	66.088005	66.440999
1400.661332	68.213792	66.446004
1400.742035	56.001958	66.451009
1399.814169	61.467332	66.456014
1398.812966	66.086354	66.461018
1398.066398	64.327350	66.466023
1397.634603	67.899213	66.471028
1397.486986	63.638193	66.476033
1396.375828	71.904684	66.481038
1395.453618	61.893766	66.486042
1394.874400	68.599665	66.491047
1394.454947	62.803540	66.496052
1393.803537	59.363328	66.501057
1392.834858	63.776266	66.506062
1392.124258	53.110609	66.511066
1391.769696	59.053741	66.516071
1391.264455	62.267141	66.521076
1390.583423	64.609884	66.526081
1389.216660	71.491248	66.531086
1388.906078	65.274664	66.536090
1388.350147	76.350454	66.541095
1388.416863	69.325635	66.546100
1386.989801	68.340322	66.551105
1386.019469	70.107354	66.556110
1385.651795	58.633424	66.561114
1384.908202	60.982535	66.566119
1384.654992	57.923747	66.571124
1384.037525	61.107017	66.576129
1383.155074	67.062360	66.581134
1382.768104	57.438227	66.586138
1381.591798	61.747766	66.591143
1380.254962	62.462851	66.596148
1380.375176	57.487730	66.601153
1379.831653	57.446917	66.606158
1379.503975	56.077244	66.611162
1378.910318	61.053590	66.616167
1377.311416	64.597088	66.621172
1376.956692	67.379743	66.626177
1376.140944	64.105420	66.631182
1375.965508	65.025893	66.636186
1375.330378	60.600443	66.641191
1374.374393	64.747934	66.646196
1373.927145	66.924746	66.651201
1373.072042	73.655770	66.656206
1372.660425	57.759047	66.661210
1372.016509	62.244284	66.666215
1371.460190	60.932696	66.671220
1370.150997	61.509637	66.676225
1369.608870	59.627226	66.681230
1369.439315	62.417656	66.686234
1369.056339	62.219499	66.691239
1367.682031	62.299585	66.696244
1366.928354	63.899276	66.701249
1366.326932	68.196460	66.706254
1365.833626	60.633198	66.711258
1365.275737	65.138050	66.716263
1364.733224	61.516578	66.721268
1363.984851	63.389690	66.726273
1362.990437	66.752352	66.731278
1362.626784	62.913560	66.736282
1362.140821	63.361030	66.741287
1361.666488	58.434002	66.746292
1361.031422	61.127284	66.751297
1360.238367	64.444030	66.756302
1359.630358	56.848697	66.761306
1358.436706	65.316012	66.766311
1357.689873	59.892893	66.771316
1357.304464	60.976409	66.776321
1356.644457	64.570760	66.781326
1356.271763	58.657696	66.786330
1355.195351	55.963632	66.791335
1354.552682	56.798305	66.796340
1354.065387	57.018251	66.801345
1353.173567	61.130683	66.806350
1353.326644	67.108493	66.811354
1352.259278	60.678058	66.816359
1351.423829	62.713703	66.821364
1350.777740	52.110037	66.826369
1349.694940	59.830514	66.831374
1349.095775	62.729221	66.836378
1348.461574	57.441159	66.841383
1347.741366	60.447029	66.846388
1347.417322	59.408694	66.851393
1346.688207	63.591954	66.856398
1346.713901	54.966480	66.861402
1345.720225	58.461641	66.866407
1344.726423	59.473654	66.871412
1344.786977	58.515134	66.876417
1343.030993	66.355985	66.881422
1342.281168	58.179040	66.886426
1341.644291	61.803378	66.891431
1341.044186	59.268165	66.896436
1340.977162	57.144962	66.901441
1340.185310	60.241646	66.906446
1340.087772	59.214666	66.911450
1338.909431	58.833734	66.916455
1338.194404	70.202004	66.921460
1337.803503	65.752909	66.926465
1336.974865	64.788717	66.931470
1335.882993	67.319422	66.936474
1335.141551	59.796669	66.941479
1334.615376	61.102827	66.946484
1334.350949	56.369201	66.951489
1333.735009	62.697721	66.956494
1333.092680	61.598615	66.961498
1332.193100	63.525641	66.966503
1331.437315	63.821550	66.971508
1331.343302	66.779830	66.976513
1330.503046	65.311599	66.981518
1329.265603	65.131040	66.986522
1328.834358	68.115472	66.991527
1328.284043	65.065313	66.996532
1327.949797	61.262937	67.001537
1326.461763	68.312302	67.006542
1325.667335	63.568356	67.011546
1325.236801	60.989907	67.016551
1324.717933	62.460201	67.021556
1324.625040	63.282469	67.026561
1324.137634	66.110734	67.031566
1323.359329	67.465580	67.036570
1322.093364	56.064129	67.041575
1321.688191	58.410179	67.046580
1321.529588	48.101606	67.051585
1320.219561	64.823053	67.056590
1318.952392	64.797578	67.061594
1319.131930	64.919952	67.066599
1318.155441	63.292291	67.071604
1317.790465	58.205634	67.076609
1317.307114	62.883641	67.081614
1316.767936	56.058866	67.086618
1315.758846	66.678960	67.091623
1315.105863	65.019602	67.096628
1314.756689	58.949761	67.101633
1312.991354	59.575594	67.106638
1312.729775	60.395163	67.111642
1312.350653	69.055400	67.116647
1312.046009	63.379757	67.121652
1311.951464	63.386427	67.126657
1310.371143	66.703747	67.131662
1309.824690	57.927153	67.136666
1309.286581	61.354201	67.141671
1308.677104	60.395915	67.146676
1307.762541	58.569770	67.151681
1306.904187	60.571054	67.156686
1306.184566	55.253020	67.161690
1305.899311	54.756311	67.166695
1305.125965	69.485719	67.171700
1304.446672	73.386917	67.176705
1303.144889	64.069395	67.181710
1302.940133	61.024817	67.186714
1302.516112	63.662240	67.191719
1301.937020	65.820182	67.196724
1301.708519	60.443729	67.201729
1300.348281	68.706294	67.206734
1299.624232	61.242936	67.211738
1299.199337	71.507249	67.216743
1298.936555	69.442425	67.221748
1297.832934	61.868793	67.226753
1296.503483	70.347131	67.231758
1296.291637	69.790094	67.236762
1295.539988	61.222305	67.241767
1295.350170	67.334597	67.246772
1295.258263	71.321546	67.251777
1294.157123	75.064447	67.256782
1293.243179	68.479083	67.261786
1292.733957	66.338428	67.266791
1292.106258	65.994682	67.271796
1291.189458	56.130891	67.276801
1289.967405	62.010176	67.281806
1289.741744	57.837918	67.286810
1289.014441	61.983374	67.291815
1288.755487	58.373762	67.296820
1288.391909	65.111429	67.301825
1287.242766	71.685570	67.306830
1286.744655	63.624220	67.311834
1285.944677	56.322281	67.316839
1285.366489	67.514368	67.321844
1284.888798	61.284567	67.326849
1283.868730	59.750817	67.331854
1282.988839	61.830788	67.336858
1282.637026	59.671872	67.341863
1282.179243	57.160458	67.346868
1281.643907	61.791711	67.351873
1280.091608	64.623081	67.356878
1280.049848	58.126030	67.361882
1279.317434	66.888193	67.366887
1278.967356	64.268343	67.371892
1278.651493	54.283917	67.376897
1277.311413	55.813492	67.381902
1276.670897	53.215736	67.386906
1276.107316	56.471496	67.391911
1275.458584	68.144585	67.396916
1274.905239	60.938180	67.401921
1273.749982	58.436046	67.406926
1273.435931	59.832598	67.411930
1272.913907	61.186600	67.416935
1272.495479	64.769995	67.421940
1271.316980	57.627593	67.426945
1270.578417	64.551423	67.431950
1270.118793	61.811784	67.436954
1269.608198	57.797644	67.441959
1268.854901	62.016234	67.446964
1267.791926	63.373640	67.451969
1266.732983	59.154970	67.456974
1266.814216	56.300239	67.461978
1266.373289	60.930723	67.466983
1266.046339	63.464692	67.471988
1265.255961	58.247986	67.476993
1264.076090	63.054712	67.481998
1263.319654	59.564216	67.487002
1263.078235	48.150410	67.492007
1262.248629	59.368561	67.497012
1261.482235	51.341705	67.502017
1260.766182	57.440668	67.507022
1260.237088	65.046235	67.512026
1259.854684	58.359621	67.517031
1258.759271	57.781756	67.522036
1257.883337	58.344154	67.527041
1257.504184	63.875072	67.532046
1257.279258	59.537698	67.537050
1256.668437	53.178730	67.542055
1255.337774	68.421949	67.547060
1254.611695	56.889807	67.552065
1254.047344	59.602175	67.557070
1253.673474	55.126100	67.562074
1253.465688	56.232894	67.567079
1252.486327	64.004358	67.572084
1251.747435	50.132951	67.577089
1250.871936	55.448461	67.582094
1250.372018	57.312208	67.587098
1249.961322	54.660901	67.592103
1248.964039	67.440848	67.597108
1248.232519	57.982695	67.602113
1247.680709	75.267079	67.607118
1247.418195	60.933993	67.612122
1246.346884	52.613964	67.617127
1245.381678	68.225648	67.622132
1244.625436	59.801546	67.627137
1244.215540	62.287351	67.632142
1243.639785	69.183707	67.637146
1243.590786	65.283165	67.642151
1242.490749	66.094712	67.647156
1241.666547	63.580510	67.652161
1241.141355	62.615698	67.657166
1240.778920	63.993299	67.662170
1239.625293	59.068908	67.667175
1238.453147	65.282274	67.672180
1238.374386	58.746168	67.677185
1237.856853	69.008181	67.682190
1237.415945	63.677966	67.687194
1236.303916	59.292348	67.692199
1235.269231	62.860862	67.697204
1235.143893	56.067876	67.702209
1234.255978	66.369220	67.707214
1233.880118	65.816583	67.712218
1233.542122	61.631194	67.717223
1232.285900	69.839255	67.722228
1231.822705	62.579530	67.727233
1231.104411	66.364259	67.732238
1230.647485	59.205694	67.737242
1230.434855	60.273452	67.742247
1229.211370	69.543619	67.747252
1228.806296	70.579197	67.752257
1227.966019	66.998460	67.757262
1226.888605	70.076553	67.762266
1226.600612	57.308945	67.767271
1225.544824	66.531454	67.772276
1225.360192	57.880027	67.777281
1224.912995	64.905548	67.782286
1224.113213	58.204744	67.787290
1223.223235	70.584237	67.792295
1222.313565	66.287522	67.797300
1221.926789	61.228293	67.802305
1221.546597	67.358571	67.807310
1220.694278	52.968985	67.812314
1219.998188	52.886813	67.817319
1219.283090	62.542019	67.822324
1218.624712	55.352426	67.827329
1217.718344	64.389097	67.832334
1216.903973	60.936158	67.837338
1216.412397	57.033238	67.842343
1216.010846	61.763557	67.847348
1215.872502	61.837724	67.852353
1214.476532	67.485103	67.857358
1213.817596	64.675389	67.862362
1213.268942	58.669318	67.867367
1212.918178	61.392883	67.872372
1212.557125	58.222316	67.877377
1211.291003	59.761744	67.882382
1210.480656	59.605982	67.887386
1209.992266	56.223544	67.892391
1209.315034	60.118079	67.897396
1209.147996	54.461128	67.902401
1207.831133	57.461409	67.907406
1207.078470	60.338252	67.912410
1206.850793	59.659989	67.917415
1205.838367	60.108008	67.922420
1205.765507	64.283525	67.927425
1204.086486	69.850691	67.932430
1203.901797	65.833652	67.937434
1203.035076	58.600787	67.942439
1202.328105	62.370553	67.947444
1202.200599	54.424184	67.952449
1201.480993	68.011155	67.957454
1201.186716	62.409538	67.962458
1200.599222	68.514918	67.967463
1199.647978	66.479163	67.972468
1199.247400	62.939198	67.977473
1198.047458	61.924529	67.982478
1197.027817	59.513664	67.987482
1196.740948	61.843809	67.992487
1196.053420	67.144514	67.997492
1196.100675	58.411154	68.002497
1194.957412	61.712094	68.007502
1194.116753	61.123783	68.012506
1193.539560	49.882734	68.017511
1192.773223	63.491517	68.022516
1192.328258	54.156021	68.027521
1191.011390	52.673109	68.032526
1190.301717	55.327867	68.037530
1190.396816	51.483971	68.042535
1189.728885	59.976949	68.047540
1189.602504	47.598902	68.052545
1188.175923	65.432102	68.057550
1187.194297	60.157371	68.062554
1187.158686	48.651897	68.067559
1186.395910	61.340378	68.072564
1185.898633	55.802730	68.077569
1184.776863	59.521944	68.082574
1184.151059	64.951812	68.087578
1183.930844	67.398434	68.092583
1182.901377	64.842023	68.097588
1182.211672	65.300316	68.102593
1181.178972	64.715678	68.107598
1180.526321	57.201443	68.112602
1180.563744	60.417070	68.117607
1179.700975	54.700829	68.122612
1179.399436	53.506294	68.127617
1178.459906	59.723653	68.132622
1177.783547	56.508792	68.137626
1177.054309	57.411200	68.142631
1176.366707	65.676639	68.147636
1175.578160	51.346805	68.152641
1174.680375	66.440523	68.157646
1174.303386	61.619217	68.162650
1173.904779	57.274090	68.167655
1173.185999	60.529196	68.172660
1172.529644	53.713064	68.177665
1171.713547	58.099908	68.182670
1171.320389	56.750147	68.187674
1170.381078	50.608484	68.192679
1168.963587	56.750582	68.197684
1168.377938	52.278412	68.202689
1167.842432	56.138816	68.207694
1167.616935	54.891395	68.212698
1167.451394	48.073331	68.217703
1166.793156	54.822367	68.222708
1166.588345	51.691762	68.227713
1165.036091	47.639292	68.232718
1164.400744	58.605119	68.237722
1164.229905	48.092226	68.242727
1162.938694	66.716553	68.247732
1162.347558	51.366129	68.252737
1161.614101	54.280738	68.257742
1161.356204	62.040783	68.262746
1160.798759	61.858700	68.267751
1159.508377	62.500365	68.272756
1158.631563	60.648051	68.277761
1158.165799	54.222820	68.282766
1157.948919	58.232344	68.287770
1157.800042	52.816619	68.292775
1156.822458	59.880849	68.297780
1155.867475	59.144760	68.302785
1155.118054	57.596670	68.307790
1154.554532	58.149408	68.312794
1154.352795	48.650309	68.317799
1153.212845	60.504995	68.322804
1152.603164	49.124658	68.327809
1151.931386	59.021514	68.332814
1151.391222	54.863252	68.337818
1150.507174	58.711892	68.342823
1149.001861	59.377335	68.347828
1148.428749	51.843964	68.352833
1148.319879	54.886884	68.357838
1147.892927	64.160406	68.362842
1147.114591	59.813198	68.367847
1146.883809	58.392612	68.372852
1146.702666	58.399903	68.377857
1145.814588	54.367920	68.382862
1145.424806	57.456965	68.387866
1144.611073	50.870671	68.392871
1143.401051	62.210410	68.397876
1142.703004	57.000815	68.402881
1141.370096	60.621985	68.407886
1141.007365	60.775230	68.412890
1140.646403	55.025970	68.417895
1139.944629	60.313723	68.422900
1139.413128	57.588775	68.427905
1138.978310	63.017916	68.432910
1137.998821	59.382487	68.437914
1137.186497	54.419817	68.442919
1136.467916	62.267030	68.447924
1136.578883	55.170713	68.452929
1135.667917	59.298687	68.457934
1134.459502	54.916971	68.462938
1133.655630	58.727018	68.467943
1132.977059	66.733163	68.472948
1132.487956	58.423210	68.477953
1132.324608	53.247979	68.482958
1131.747503	53.334515	68.487962
1131.112695	54.512851	68.492967
1129.999286	60.740254	68.497972
1129.538460	53.756052	68.502977
1129.098790	60.730550	68.507982
1127.864996	60.219039	68.512986
1127.559649	53.926995	68.517991
1126.820895	61.374262	68.522996
1126.435889	48.586189	68.528001
1125.612540	62.822860	68.533006
1124.529210	59.748345	68.538010
1124.217962	52.090013	68.543015
1123.453874	61.723613	68.548020
1123.008314	53.833291	68.553025
1122.151335	56.399601	68.558030
1121.304823	55.039845	68.563034
1120.751540	48.536849	68.568039
1120.149032	61.627341	68.573044
1119.963428	50.748316	68.578049
1118.997698	54.020055	68.583054
1117.873837	50.292517	68.588058
1117.586601	50.306133	68.593063
1116.637661	56.599712	68.598068
1116.771500	56.930025	68.603073
1115.725897	49.792155	68.608078
1114.732894	59.894402	68.613082
1114.564784	42.298650	68.618087
1113.692390	51.805928	68.623092
1112.815769	50.963671	68.628097
1111.775362	55.121706	68.633102
1111.134612	51.307894	68.638106
1110.798169	51.927932	68.643111
1110.380597	51.271533	68.648116
1110.096338	49.007915	68.653121
1109.432997	54.534206	68.658126
1108.407262	61.549849	68.663130
1107.925858	50.981594	68.668135
1106.729677	62.104241	68.673140
1105.764011	53.259744	68.678145
1105.254074	49.798516	68.683150
1104.899680	51.328687	68.688154
1104.660921	46.002566	68.693159
1104.071185	54.002180	68.698164
1103.656775	46.321257	68.703169
1102.256357	48.612352	68.708174
1101.572623	54.547510	68.713178
1101.393169	46.506241	68.718183
1100.622538	51.655003	68.723188
1099.513033	44.397037	68.728193
1098.977390	45.469584	68.733198
1098.348586	49.445436	68.738202
1098.180571	51.791939	68.743207
1097.031467	50.213620	68.748212
1096.528859	54.255491	68.753217
1095.592273	51.988315	68.758222
1095.143315	53.299428	68.763226
1094.769267	52.008373	68.768231
1093.465903	57.000082	68.773236
1092.715533	57.080767	68.778241
1092.153898	52.368852	68.783246
1091.825189	49.623002	68.788250
1091.477750	47.018117	68.793255
1090.546167	54.088686	68.798260
1089.545097	47.901176	68.803265
1088.757096	51.167747	68.808270
1088.180749	48.222341	68.813274
1088.135697	48.076864	68.818279
1087.701586	49.235837	68.823284
1086.814103	53.844113	68.828289
1085.913848	52.917491	68.833294
1085.073320	51.851175	68.838298
1084.783043	51.071144	68.843303
1083.570110	63.599092	68.848308
1082.590592	54.582903	68.853313
1082.145659	60.637823	68.858318
1081.891565	61.797945	68.863322
1082.054942	57.049903	68.868327
1080.661064	57.338277	68.873332
1079.847429	51.773113	68.878337
1079.179405	58.280292	68.883342
1078.619567	54.696170	68.888346
1078.697288	48.820489	68.893351
1077.248703	57.683976	68.898356
1076.751763	53.825809	68.903361
1076.034066	54.814276	68.908366
1075.333363	61.596248	68.913370
1074.298159	56.706493	68.918375
1073.341249	64.222303	68.923380
1072.937011	56.623714	68.928385
1072.642971	65.442261	68.933390
1072.099247	65.265338	68.938394
1071.868655	59.353242	68.943399
1070.616963	63.754692	68.948404
1069.782853	57.865025	68.953409
1069.159586	56.948604	68.958414
1068.686633	57.137307	68.963418
1068.207841	53.768639	68.968423
1066.990125	64.084627	68.973428
1066.407340	49.733409	68.978433
1065.874207	53.595387	68.983438
1065.528999	55.862897	68.988442
1065.095087	57.889426	68.993447
1063.812377	58.411386	68.998452
1063.173356	51.794404	69.003457
1062.916529	60.558025	69.008462
1062.222126	62.985591	69.013466
1062.194687	46.875154	69.018471
1060.497475	55.314663	69.023476
1059.996779	57.378284	69.028481
1059.681873	61.757472	69.033486
1058.775350	48.945829	69.038490
1058.094079	51.878749	69.043495
1057.224796	63.727753	69.048500
1057.386414	60.484673	69.053505
1056.448249	56.003810	69.058510
1054.925668	53.410695	69.063514
1054.361067	56.191803	69.068519
1053.756353	63.571519	69.073524
1053.274089	53.000264	69.078529
1052.635499	63.828499	69.083534
1052.214246	62.266861	69.088538
1052.245927	57.790438	69.093543
1051.154408	66.661866	69.098548
1050.478191	60.693851	69.103553
1049.641707	50.688888	69.108558
1048.592980	55.720286	69.113562
1047.851239	55.854761	69.118567
1046.937805	60.975883	69.123572
1046.748255	54.139837	69.128577
1046.345392	60.095190	69.133582
1045.865361	54.908278	69.138586
1045.311098	54.672771	69.143591
1044.233371	61.801136	69.148596
1043.968514	62.030782	69.153601
1043.267485	51.896445	69.158606
1042.077016	60.646665	69.163610
1041.645043	57.324059	69.168615
1040.918103	62.218650	69.173620
1040.480000	67.141936	69.178625
1039.488120	58.366283	69.183630
1038.800668	56.840758	69.188634
1038.365535	56.627087	69.193639
1037.459269	62.638253	69.198644
1037.307337	50.445779	69.203649
1036.084566	56.895201	69.208654
1035.227164	56.699371	69.213658
1034.938504	46.222464	69.218663
1033.842808	58.763098	69.223668
1033.797734	62.737676	69.228673
1033.252271	60.662074	69.233678
1032.684695	55.287272	69.238682
1031.540363	53.673811	69.243687
1030.519999	49.876076	69.248692
1030.550249	56.421962	69.253697
1030.404538	51.967236	69.258702
1029.022162	58.224134	69.263706
1028.445690	50.404010	69.268711
1027.585553	59.319889	69.273716
1027.630845	59.581682	69.278721
1026.279101	53.444371	69.283726
1025.430929	62.367675	69.288730
1024.824818	55.098123	69.293735
1024.242823	65.972718	69.298740
1023.999804	58.930708	69.303745
1023.204068	51.075505	69.308750
1022.166226	61.831591	69.313754
1021.746871	61.529171	69.318759
1021.339726	63.344288	69.323764
1020.859110	54.798048	69.328769
1019.538196	59.927772	69.333774
1018.575521	67.636804	69.338778
1018.355303	61.330983	69.343783
1017.832775	65.163125	69.348788
1017.361537	51.118459	69.353793
1016.988136	55.292542	69.358798
1015.663969	55.489658	69.363802
1015.038320	50.009548	69.368807
1014.733486	58.612843	69.373812
1013.959144	56.010811	69.378817
1013.061518	60.309009	69.383822
1012.327429	54.547878	69.388826
1012.099961	51.750359	69.393831
1011.467796	57.692482	69.398836
1010.779300	55.576249	69.403841
1009.447011	56.793126	69.408846
1008.790640	52.076133	69.413850
1008.465920	50.884396	69.418855
1007.961306	62.162557	69.423860
1007.941848	60.914201	69.428865
1006.634590	50.728962	69.433870
1005.553428	54.310603	69.438874
1005.258785	60.703322	69.443879
1004.773402	62.666831	69.448884
1004.306522	56.726922	69.453889
1003.265042	60.518074	69.458894
1002.727463	56.701216	69.463898
1002.289633	56.115398	69.468903
1001.033857	52.700598	69.473908
1000.009803	46.221013	69.478913
999.468412	51.899707	69.483918
998.692040	52.312474	69.488922
998.762095	50.554605	69.493927
998.094157	62.698324	69.498932
998.317996	50.010870	69.503937
997.409912	44.585843	69.508942
996.157175	54.332730	69.513946
995.703800	48.900881	69.518951
994.477463	55.622880	69.523956
993.843001	50.082313	69.528961
993.116957	51.897177	69.533966
992.719372	58.570010	69.538970
992.489413	48.955380	69.543975
991.564766	58.041773	69.548980
990.702094	49.887794	69.553985
990.216501	45.866654	69.558990
989.391117	54.737899	69.563994
989.161060	52.525004	69.568999
987.888019	58.821211	69.574004
987.410365	50.111455	69.579009
986.894097	54.738272	69.584014
985.994294	57.546003	69.589018
985.390251	52.498754	69.594023
984.502362	61.019542	69.599028
983.824885	56.616414	69.604033
983.785178	52.959021	69.609038
983.055547	58.660877	69.614042
982.249423	60.942593	69.619047
981.139925	64.603694	69.624052
980.710974	56.844756	69.629057
980.277795	61.129337	69.634062
979.945944	55.362482	69.639066
978.973051	54.396218	69.644071
977.810430	59.272275	69.649076
977.515757	59.418218	69.654081
977.078811	57.021687	69.659086
976.536468	55.230150	69.664090
975.428410	52.092807	69.669095
974.610271	61.923555	69.674100
974.129092	54.743139	69.679105
973.708543	58.996348	69.684110
972.915623	58.483580	69.689114
972.084326	50.428833	69.694119
971.440774	51.454351	69.699124
970.981655	54.095038	69.704129
970.706505	55.350739	69.709134
969.560684	61.100585	69.714138
968.764740	58.757642	69.719143
968.026672	60.265507	69.724148
967.415438	57.188730	69.729153
967.308714	61.529109	69.734158
966.494322	62.679012	69.739162
966.012681	54.138879	69.744167
965.107028	57.032873	69.749172
964.530547	51.148451	69.754177
963.452062	62.568311	69.759182
962.228372	56.032137	69.764186
961.804979	57.551634	69.769191
961.180773	53.954872	69.774196
961.130162	61.273246	69.779201
960.936280	54.217305	69.784206
960.042137	60.158117	69.789210
959.272858	47.907972	69.794215
958.405061	49.284905	69.799220
958.124865	49.117729	69.804225
957.311883	51.575481	69.809230
956.296086	50.271982	69.814234
955.897844	54.519791	69.819239
955.110180	54.857135	69.824244
953.955485	53.432958	69.829249
953.499449	57.106092	69.834254
952.752246	55.966583	69.839258
952.271396	49.665544	69.844263
951.788548	60.561442	69.849268
951.309183	56.682520	69.854273
951.081478	57.098824	69.859278
949.568345	58.085780	69.864282
949.371978	53.606974	69.869287
948.555291	53.284981	69.874292
947.952052	57.596714	69.879297
946.847954	59.513435	69.884302
945.962891	63.475167	69.889306
945.630679	42.976394	69.894311
944.965503	53.806414	69.899316
944.800522	49.193556	69.904321
944.752351	51.131530	69.909326
943.329248	50.298823	69.914330
942.931775	53.343406	69.919335
942.019362	67.783222	69.924340
941.117248	56.563142	69.929345
940.563430	54.048480	69.934350
939.496521	63.923416	69.939354
939.645404	56.514315	69.944359
938.118769	54.679788	69.949364
937.595091	60.042841	69.954369
937.183213	54.103391	69.959374
936.381871	63.537339	69.964378
936.257418	52.668789	69.969383
935.722897	60.141482	69.974388
934.636310	61.397609	69.979393
933.797835	53.541063	69.984398
932.958812	66.884814	69.989402
933.029204	52.262693	69.994407
931.631808	63.733623	69.999412
930.736971	62.093245	70.004417
930.374842	63.705669	70.009422
929.587424	60.862746	70.014426
929.547026	53.846045	70.019431
928.851505	55.524645	70.024436
928.422456	56.234761	70.029441
927.350789	49.360344	70.034446
926.445483	54.438247	70.039450
926.215706	57.315961	70.044455
925.703153	54.165847	70.049460
924.801496	56.784440	70.054465
924.279550	45.335456	70.059470
923.449925	51.670198	70.064474
922.879066	54.051356	70.069479
921.640947	55.874200	70.074484
920.971205	51.620936	70.079489
920.599440	53.536967	70.084494
919.953506	54.586582	70.089498
919.563994	47.257855	70.094503
919.114691	51.565722	70.099508
918.079489	48.601434	70.104513
917.582478	52.280007	70.109518
916.715240	56.415127	70.114522
916.509103	48.202801	70.119527
915.047178	58.402350	70.124532
914.220190	58.069102	70.129537
913.814598	54.518980	70.134542
913.706892	64.016095	70.139546
913.637458	53.434162	70.144551
912.662200	57.078204	70.149556
911.567438	53.065489	70.154561
911.181383	54.047307	70.159566
909.847534	57.860523	70.164570
909.255906	48.960314	70.169575
908.078055	60.774150	70.174580
907.591671	55.233497	70.179585
907.418161	50.317778	70.184590
906.802062	55.166950	70.189594
906.955038	46.265523	70.194599
906.137803	56.240583	70.199604
904.793491	57.695586	70.204609
904.077430	55.472388	70.209614
903.218427	59.540181	70.214618
903.392283	52.718881	70.219623
901.919091	57.857737	70.224628
901.076741	53.127619	70.229633
900.894194	51.854306	70.234638
900.242132	53.283900	70.239642
899.963221	41.489368	70.244647
898.940947	51.136010	70.249652
898.240638	47.372303	70.254657
897.958424	50.245577	70.259662
897.135626	49.155733	70.264666
895.953911	47.549105	70.269671
895.251602	51.100218	70.274676
894.727534	51.125991	70.279681
894.725465	44.633625	70.284686
893.965159	55.510333	70.289690
893.141120	46.350740	70.294695
892.620636	54.958203	70.299700
891.762995	57.609129	70.304705
891.308019	58.626042	70.309710
889.749463	51.703980	70.314714
889.258899	42.433988	70.319719
888.560018	47.589822	70.324724
888.411205	49.220971	70.329729
887.868097	50.763740	70.334734
887.258251	61.449691	70.339738
886.578852	53.193300	70.344743
885.273833	61.078999	70.349748
884.925696	53.057961	70.354753
884.670694	51.748509	70.359758
883.805524	61.116421	70.364762
883.240226	47.779444	70.369767
882.271784	51.245095	70.374772
881.560688	54.349713	70.379777
881.516014	51.978766	70.384782
880.202809	54.217089	70.389786
879.841932	52.075553	70.394791
878.857486	60.746301	70.399796
878.360910	56.204452	70.404801
878.505830	45.794224	70.409806
877.109091	61.738755	70.414810
876.434944	54.917837	70.419815
876.069320	55.231852	70.424820
875.302600	56.070462	70.429825
874.525379	52.789249	70.434830
873.553106	49.014894	70.439834
873.321922	50.587129	70.444839
872.905888	55.675575	70.449844
872.044566	53.104651	70.454849
871.085397	53.714527	70.459854
870.147690	58.667732	70.464858
869.914037	46.767956	70.469863
869.482545	60.163473	70.474868
868.714101	54.323394	70.479873
867.587642	55.616757	70.484878
866.640750	63.891886	70.489882
866.349556	51.801052	70.494887
866.086469	55.056688	70.499892
865.312733	54.923527	70.504897
864.950199	47.775704	70.509902
863.566708	60.943906	70.514906
863.490491	50.774831	70.519911
863.091508	59.913693	70.524916
861.925330	54.579479	70.529921
861.160189	49.576424	70.534926
860.047204	57.078332	70.539930
859.683829	53.152321	70.544935
859.214389	54.483144	70.549940
858.890568	52.260267	70.554945
858.355736	53.308622	70.559950
857.114039	49.318327	70.564954
856.379960	47.329528	70.569959
856.026909	51.988392	70.574964
855.669571	61.052626	70.579969
855.231791	52.245674	70.584974
853.655964	60.141449	70.589978
853.167240	57.005420	70.594983
852.851643	53.682246	70.599988
852.074300	59.182298	70.604993
851.554408	50.818468	70.609998
850.431389	52.372942	70.615002
850.014365	47.699059	70.620007
849.488111	61.695776	70.625012
848.866675	52.082696	70.630017
848.134187	51.595912	70.635022
847.260487	43.180590	70.640026
847.008430	47.626376	70.645031
846.368457	50.907884	70.650036
845.302421	57.889017	70.655041
844.330599	56.971148	70.660046
843.450844	56.229341	70.665050
843.463057	52.878439	70.670055
842.784579	60.616963	70.675060
842.492103	60.666228	70.680065
841.508266	53.919678	70.685070
840.545368	58.498275	70.690074
840.646608	45.438702	70.695079
840.096490	56.456243	70.700084
838.941336	58.217924	70.705089
838.097968	57.491989	70.710094
837.309421	60.917363	70.715098
837.049579	62.698577	70.720103
835.623673	57.756602	70.725108
835.010804	64.519600	70.730113
834.776809	60.370519	70.735118
834.216696	59.687642	70.740122
833.810133	55.230639	70.745127
833.419070	59.145268	70.750132
832.125586	66.147998	70.755137
831.532700	61.074391	70.760142
830.962913	59.781362	70.765146
830.624327	63.515302	70.770151
829.400877	57.430289	70.775156
828.551742	59.639265	70.780161
828.379081	52.911662	70.785166
827.571958	61.700061	70.790170
827.209326	61.413599	70.795175
825.914437	58.144884	70.800180
825.295122	59.761894	70.805185
824.773747	48.375593	70.810190
824.303937	53.865993	70.815194
823.902754	62.608544	70.820199
823.193722	60.362051	70.825204
822.183919	59.655944	70.830209
821.804311	57.354998	70.835214
821.334087	62.760609	70.840218
820.722467	56.362390	70.845223
819.451445	67.358955	70.850228
818.560282	64.460011	70.855233
818.411944	52.426421	70.860238
817.872984	61.842668	70.865242
817.647686	58.384825	70.870247
816.422423	65.157989	70.875252
815.851988	58.965862	70.880257
815.174844	57.682146	70.885262
813.633961	59.740023	70.890266
812.786735	56.031099	70.895271
812.472029	58.626537	70.900276
812.427321	51.749130	70.905281
812.262558	58.657596	70.910286
811.523757	58.311234	70.915290
810.655090	56.779682	70.920295
809.882014	65.019124	70.925300
808.846371	70.439487	70.930305
809.078215	55.896695	70.935310
808.030036	65.840276	70.940314
806.926051	54.412856	70.945319
806.005564	51.317636	70.950324
805.364482	54.168309	70.955329
805.317330	52.524854	70.960334
805.011065	52.082300	70.965338
803.674549	50.434715	70.970343
803.229109	50.855954	70.975348
802.591762	58.357709	70.980353
802.143147	53.298474	70.985358
800.968106	61.352177	70.990362
800.331139	53.169454	70.995367
799.565534	51.523940	71.000372
798.955513	58.099354	71.005377
798.916151	54.629796	71.010382
798.052710	57.177130	71.015386
797.034152	55.555209	71.020391
796.316459	61.203725	71.025396
795.576411	61.077830	71.030401
795.329654	58.406387	71.035406
794.929891	57.615526	71.040410
794.053398	53.022721	71.045415
793.340664	53.832360	71.050420
792.673023	56.052882	71.055425
792.346006	54.512626	71.060430
791.192808	64.394070	71.065434
790.446271	56.035522	71.070439
789.998471	59.599102	71.075444
789.273096	52.480285	71.080449
788.872230	61.423690	71.085454
787.675921	58.082051	71.090458
786.976450	53.149073	71.095463
786.353385	59.206094	71.100468
786.123591	61.414376	71.105473
785.902073	45.535778	71.110478
784.701944	58.467722	71.115482
784.205780	60.135085	71.120487
783.269777	61.423868	71.125492
782.365957	66.637321	71.130497
782.252290	57.451984	71.135502
780.864667	65.943927	71.140506
780.387076	52.675234	71.145511
780.026634	65.140077	71.150516
779.348053	60.287594	71.155521
779.468463	62.206953	71.160526
778.031922	71.181727	71.165530
777.063213	60.310189	71.170535
776.791201	61.846398	71.175540
776.314022	62.768050	71.180545
775.608891	54.414650	71.185550
774.328616	71.067896	71.190554
773.940630	64.808602	71.195559
773.636651	65.166141	71.200564
772.971951	60.066953	71.205569
772.184582	59.729311	71.210574
771.399099	57.343957	71.215578
770.748373	60.437853	71.220583
770.374773	61.424653	71.225588
769.425780	65.134874	71.230593
768.594835	55.975703	71.235598
767.853752	55.420145	71.240602
767.346942	59.295396	71.245607
766.725199	55.088409	71.250612
766.568294	61.734621	71.255617
765.886762	50.252616	71.260622
765.012307	60.482212	71.265626
764.560747	56.087791	71.270631
763.708303	53.243015	71.275636
762.409584	59.691288	71.280641
762.273761	52.493591	71.285646
761.032671	57.685875	71.290650
760.613657	49.590558	71.295655
760.557081	51.227618	71.300660
759.554660	55.071721	71.305665
758.726894	48.082946	71.310670
757.740360	59.153143	71.315674
757.542406	56.920555	71.320679
757.153209	54.159048	71.325684
756.457603	55.614670	71.330689
755.612487	44.860524	71.335694
754.649621	53.707575	71.340698
754.400851	53.932506	71.345703
753.809603	57.465400	71.350708
752.933131	61.753300	71.355713
751.769765	52.769099	71.360718
750.929438	60.604429	71.365722
750.819671	51.171339	71.370727
750.700158	48.624543	71.375732
750.138554	59.687866	71.380737
749.855184	54.610988	71.385742
748.585189	61.193284	71.390746
747.996489	46.743702	71.395751
747.165027	53.476255	71.400756
746.222951	49.948586	71.405761
745.460184	49.823828	71.410766
744.871359	52.624505	71.415770
744.558873	50.268257	71.420775
744.142986	46.820968	71.425780
742.840458	55.075322	71.430785
742.525122	46.991457	71.435790
741.861156	60.497051	71.440794
741.270053	50.766701	71.445799
740.773628	52.770014	71.450804
739.528222	54.516784	71.455809
739.471141	54.758218	71.460814
738.059795	54.830219	71.465818
737.381143	50.891920	71.470823
736.919424	54.279080	71.475828
736.256226	59.092520	71.480833
735.921830	45.814313	71.485838
735.652638	55.714446	71.490842
734.459452	53.168428	71.495847
733.593732	50.957083	71.500852
733.232099	47.678912	71.505857
732.992416	41.255684	71.510862
731.488480	52.328069	71.515866
730.560148	47.881127	71.520871
730.227000	51.462171	71.525876
729.240772	54.104756	71.530881
729.106150	39.176764	71.535886
728.749457	51.743577	71.540890
728.240983	49.142236	71.545895
727.384008	41.686792	71.550900
726.690497	53.329650	71.555905
726.233989	45.565614	71.560910
725.170833	52.563636	71.565914
724.181657	47.092965	71.570919
723.906134	46.672780	71.575924
722.844905	51.898203	71.580929
722.666256	41.458953	71.585934
722.155944	45.447692	71.590938
721.342827	53.107053	71.595943
720.835164	47.862957	71.600948
719.933570	53.959800	71.605953
719.584645	48.271692	71.610958
718.559785	53.018412	71.615962
717.836390	52.509960	71.620967
717.314855	39.034492	71.625972
716.350546	43.787809	71.630977
716.134766	41.783267	71.635982
715.144084	47.595387	71.640986
714.617295	45.950817	71.645991
714.127489	49.695664	71.650996
713.295688	48.177552	71.656001
713.133796	38.248564	71.661006
711.959564	54.324715	71.666010
711.200814	46.245769	71.671015
710.854655	41.778044	71.676020
710.141631	41.279659	71.681025
709.580140	38.777005	71.686030
708.069984	49.764016	71.691034
707.601640	46.661226	71.696039
707.389779	43.317141	71.701044
706.454168	43.820781	71.706049
706.354464	36.145621	71.711054
705.725415	45.664918	71.716058
704.583233	43.560148	71.721063
703.900430	45.783671	71.726068
703.164643	56.020300	71.731073
703.177603	50.803853	71.736078
701.877132	51.811685	71.741082
701.449907	40.132200	71.746087
700.862716	42.366579	71.751092
700.086784	48.978312	71.756097
700.096304	47.365018	71.761102
698.562346	51.208616	71.766106
698.036472	47.289150	71.771111
697.592924	43.232825	71.776116
696.716938	54.598672	71.781121
696.699656	43.513657	71.786126
695.639806	51.315150	71.791130
694.522471	43.493813	71.796135
694.324954	44.806879	71.801140
693.708047	47.325018	71.806145
692.735126	45.465975	71.811150
691.772304	54.196979	71.816154
690.975120	58.744841	71.821159
691.200907	46.162474	71.826164
690.061975	58.246360	71.831169
690.154349	41.541556	71.836174
689.046452	59.502164	71.841178
688.288545	52.707083	71.846183
687.857582	48.991214	71.851188
686.790750	47.839801	71.856193
686.415190	49.168370	71.861198
685.512497	54.942923	71.866202
685.201977	51.695472	71.871207
684.192701	49.366633	71.876212
682.892548	54.123812	71.881217
682.427801	50.173745	71.886222
681.804753	58.443540	71.891226
681.688481	54.111685	71.896231
681.096760	49.240792	71.901236
680.763416	53.498412	71.906241
679.949121	49.805981	71.911246
679.321717	56.811066	71.916250
678.599428	53.983481	71.921255
677.951987	52.854952	71.926260
676.404657	55.708535	71.931265
675.710423	42.299764	71.936270
674.974052	56.170632	71.941274
674.863498	59.336592	71.946279
674.574539	47.320016	71.951284
674.022488	51.502611	71.956289
673.779924	41.370749	71.961294
672.706948	55.360858	71.966298
672.003562	48.126993	71.971303
671.068861	48.015519	71.976308
669.797410	49.455732	71.981313
669.487449	43.393873	71.986318
668.848320	50.858439	71.991322
668.350727	60.243126	71.996327
668.262272	53.241391	72.001332
667.227505	47.887882	72.006337
666.588497	42.323292	72.011342
665.463893	48.767407	72.016346
665.177075	52.338147	72.021351
664.799133	54.451424	72.026356
663.739780	53.509117	72.031361
662.981271	43.932200	72.036366
662.426294	58.549976	72.041370
662.302471	52.899885	72.046375
661.094821	50.433335	72.051380
659.990258	51.881273	72.056385
659.761493	43.534316	72.061390
659.000508	53.165428	72.066394
658.720678	49.700761	72.071399
658.441228	54.017434	72.076404
657.164215	61.288937	72.081409
656.897399	50.165756	72.086414
655.873662	53.035425	72.091418
654.869579	52.093125	72.096423
654.333567	46.050653	72.101428
653.405622	52.881845	72.106433
652.883497	46.137560	72.111438
652.502843	51.916622	72.116442
651.950010	49.592876	72.121447
651.737848	50.340457	72.126452
650.330115	49.691116	72.131457
650.045146	48.167353	72.136462
649.343912	44.639496	72.141466
648.844643	41.215190	72.146471
647.938385	50.509631	72.151476
646.676436	55.966813	72.156481
646.598170	50.499960	72.161486
645.998783	54.931838	72.166490
645.342048	55.609542	72.171495
645.262301	53.834316	72.176500
643.815788	53.677908	72.181505
643.028145	45.621691	72.186510
643.054595	56.443351	72.191514
642.122026	48.029089	72.196519
641.110669	46.895417	72.201524
640.013941	56.108817	72.206529
639.951766	46.838897	72.211534
639.504002	49.472924	72.216538
639.101531	58.377128	72.221543
638.540742	45.910581	72.226548
637.500977	45.983683	72.231553
636.986389	44.123492	72.236558
636.012050	47.215609	72.241562
634.943044	55.535757	72.246567
635.199285	45.242261	72.251572
634.416327	55.136862	72.256577
633.869064	53.058071	72.261582
632.623296	46.763803	72.266586
631.859468	41.753470	72.271591
631.785598	41.048493	72.276596
630.331739	46.885508	72.281601
629.428432	47.029570	72.286606
629.004017	44.540545	72.291610
628.778579	48.170239	72.296615
628.341363	45.069626	72.301620
627.426787	54.108537	72.306625
627.350307	47.396057	72.311630
626.363858	59.514217	72.316634
625.320889	58.363465	72.321639
624.907071	48.108193	72.326644
624.029824	64.495431	72.331649
623.635802	53.258661	72.336654
622.331469	55.538157	72.341658
621.894374	55.492219	72.346663
621.742732	45.914753	72.351668
620.896518	50.820343	72.356673
620.669490	47.875156	72.361678
619.436815	53.784801	72.366682
618.701184	52.419563	72.371687
618.206947	53.072587	72.376692
617.699178	61.534992	72.381697
617.366628	52.233635	72.386702
616.008580	50.559007	72.391706
615.356128	50.057758	72.396711
615.257866	44.618019	72.401716
614.507640	50.770250	72.406721
613.186724	53.209686	72.411726
612.387807	54.246867	72.416730
611.699608	55.139559	72.421735
611.443819	50.233621	72.426740
610.903272	51.582568	72.431745
610.898340	52.818038	72.436750
609.947174	51.708401	72.441754
608.656003	57.900819	72.446759
608.522314	44.439051	72.451764
607.891407	51.267116	72.456769
607.343539	38.980332	72.461774
606.482167	44.218105	72.466778
605.559535	52.135830	72.471783
605.648834	47.262343	72.476788
603.893424	50.753931	72.481793
603.086355	42.193056	72.486798
602.508941	46.734848	72.491802
601.572640	53.219735	72.496807
601.738591	49.503048	72.501812
601.215715	58.028431	72.506817
601.134026	53.361859	72.511822
600.101169	53.665878	72.516826
599.082347	49.906275	72.521831
599.025217	44.344629	72.526836
597.685853	48.878424	72.531841
596.671347	51.776126	72.536846
595.864728	57.849213	72.541850
595.307821	56.582428	72.546855
595.176747	53.154249	72.551860
594.929278	53.835650	72.556865
594.205934	52.807765	72.561870
593.316167	46.695264	72.566874
592.320964	45.289641	72.571879
592.125065	39.500734	72.576884
590.888862	46.075685	72.581889
589.947701	49.090287	72.586894
589.342853	47.384111	72.591898
589.061954	48.919086	72.596903
588.862377	47.745413	72.601908
588.092068	49.467262	72.606913
587.175702	54.301592	72.611918
586.556664	55.792272	72.616922
586.022980	50.394770	72.621927
585.935213	56.875978	72.626932
584.058340	49.324144	72.631937
583.578775	46.451043	72.636942
583.039557	50.736834	72.641946
582.349967	51.499118	72.646951
582.582987	45.429100	72.651956
581.552584	48.444784	72.656961
580.318065	41.974539	72.661966
579.468384	54.280042	72.666970
578.765759	50.715728	72.671975
578.931600	47.776253	72.676980
578.066396	47.301199	72.681985
577.345179	48.136794	72.686990
576.531328	52.284914	72.691994
576.107434	45.262512	72.696999
575.657592	47.513631	72.702004
574.784138	46.388713	72.707009
574.160157	52.221309	72.712014
573.683246	51.151993	72.717018
572.553188	50.042227	72.722023
571.733263	42.862695	72.727028
570.942536	50.893605	72.732033
570.816873	59.054894	72.737038
569.899665	49.395459	72.742042
569.337582	54.168300	72.747047
568.833596	50.924011	72.752052
567.837743	57.619227	72.757057
567.250285	47.351878	72.762062
566.662128	48.426766	72.767066
566.254538	49.189284	72.772071
565.389975	46.391230	72.777076
564.606795	53.312095	72.782081
564.024371	45.874778	72.787086
563.521197	48.010701	72.792090
562.776085	48.510937	72.797095
562.159852	53.271741	72.802100
561.176719	50.230334	72.807105
561.021160	44.741999	72.812110
560.485900	55.342541	72.817114
559.377957	51.376784	72.822119
558.736648	48.685338	72.827124
557.804426	55.282815	72.832129
557.141268	55.343903	72.837134
557.252260	57.567610	72.842138
556.207537	56.800048	72.847143
554.992173	48.083365	72.852148
554.668958	59.518317	72.857153
554.313560	53.051384	72.862158
553.490990	63.021462	72.867162
553.198254	61.051034	72.872167
552.258230	59.595309	72.877172
551.459832	58.657260	72.882177
551.147228	48.723719	72.887182
550.044074	62.810588	72.892186
549.129340	58.883959	72.897191
548.466691	52.118376	72.902196
547.579644	54.123113	72.907201
547.629085	57.712421	72.912206
547.145308	59.282160	72.917210
546.573211	55.563256	72.922215
545.939488	59.119234	72.927220
544.596071	59.640679	72.932225
544.565791	55.832884	72.937230
543.930146	56.207399	72.942234
542.689302	55.223986	72.947239
542.370135	47.547759	72.952244
541.494428	52.816813	72.957249
541.193789	47.270843	72.962254
540.221092	47.870075	72.967258
539.094605	59.183337	72.972263
539.051450	48.540904	72.977268
537.920869	52.895659	72.982273
537.664169	54.191241	72.987278
537.497875	52.310854	72.992282
536.602503	54.805281	72.997287
535.837099	51.046875	73.002292
535.389104	54.668918	73.007297
534.452920	49.305263	73.012302
533.377159	58.104188	73.017306
532.810708	55.213613	73.022311
532.802291	56.993201	73.027316
531.538293	61.975918	73.032321
530.522260	53.949386	73.037326
529.914711	62.747030	73.042330
529.333230	60.481100	73.047335
529.138757	60.511222	73.052340
528.249803	52.863552	73.057345
528.154743	49.395262	73.062350
527.687167	51.876384	73.067354
526.433569	53.685000	73.072359
525.864492	49.346672	73.077364
525.010199	60.842625	73.082369
524.443229	51.390805	73.087374
523.672990	52.309014	73.092378
522.902131	56.258734	73.097383
522.814269	54.255967	73.102388
522.142522	55.484123	73.107393
520.975636	58.795954	73.112398
520.250974	53.639595	73.117402
519.808704	58.766494	73.122407
519.625052	56.228726	73.127412
518.374461	59.831990	73.132417
517.409897	52.474763	73.137422
517.027513	52.319597	73.142426
516.474479	61.623396	73.147431
516.273513	47.580308	73.152436
514.931046	49.415207	73.157441
514.238814	56.992692	73.162446
513.570853	62.170501	73.167450
513.206778	59.339982	73.172455
512.978858	51.131837	73.177460
512.092242	59.499693	73.182465
511.178325	56.239606	73.187470
510.380917	52.637469	73.192474
509.899281	57.060628	73.197479
509.544765	47.307162	73.202484
508.115584	55.977580	73.207489
507.620269	55.118650	73.212494
507.205600	57.819643	73.217498
506.525151	50.803319	73.222503
506.340142	48.415777	73.227508
505.297372	57.190105	73.232513
504.542231	50.615634	73.237518
503.632224	50.484173	73.242522
503.237026	52.283460	73.247527
503.290318	42.792074	73.252532
502.242638	47.953239	73.257537
501.688871	46.392262	73.262542
500.830491	52.371996	73.267546
499.402932	57.567471	73.272551
498.877090	53.697367	73.277556
498.034476	52.992681	73.282561
498.191342	56.633837	73.287566
497.827644	53.761812	73.292570
497.525698	61.231373	73.297575
496.158557	52.650052	73.302580
495.076514	55.500138	73.307585
494.773864	48.626699	73.312590
494.296782	41.716447	73.317594
493.354966	53.087270	73.322599
492.359401	56.938138	73.327604
491.555178	56.083593	73.332609
491.336612	53.498918	73.337614
490.871657	49.747060	73.342618
490.322966	58.214108	73.347623
489.390350	44.114439	73.352628
488.508329	51.960879	73.357633
487.940963	46.181558	73.362638
487.593582	42.225224	73.367642
486.952554	45.767852	73.372647
485.817597	45.858484	73.377652
485.139249	51.038861	73.382657
484.492840	51.186689	73.387662
484.012010	47.107966	73.392666
483.855009	60.289067	73.397671
483.257212	51.984052	73.402676
481.852665	60.584734	73.407681
481.150180	54.186760	73.412686
480.877421	57.619710	73.417690
480.439699	57.929530	73.422695
480.087929	53.100444	73.427700
479.000353	54.367099	73.432705
478.134205	55.905662	73.437710
477.968992	47.975708	73.442714
476.707229	56.430350	73.447719
475.792534	49.489303	73.452724
475.091146	55.275174	73.457729
474.916533	53.563970	73.462734
474.629476	51.217599	73.467738
473.876831	56.315584	73.472743
472.786097	55.040035	73.477748
471.970498	55.981812	73.482753
471.617741	52.031530	73.487758
471.248469	60.740188	73.492762
470.046285	57.511745	73.497767
469.640633	46.684744	73.502772
468.720253	53.069819	73.507777
467.936463	55.459878	73.512782
467.948042	55.526532	73.517786
466.956089	57.974762	73.522791
466.066402	60.105090	73.527796
465.382076	58.722796	73.532801
465.178479	56.787625	73.537806
465.098747	48.933019	73.542810
463.785161	50.789033	73.547815
463.290700	55.568449	73.552820
462.388896	51.680677	73.557825
461.577798	46.680453	73.562830
460.709994	60.650817	73.567834
459.718990	65.255209	73.572839
459.466117	47.276650	73.577844
458.853734	57.667001	73.582849
458.783456	48.337309	73.587854
458.271927	51.383304	73.592858
456.637199	58.718116	73.597863
456.447906	55.194139	73.602868
455.737541	56.717062	73.607873
454.953377	50.608997	73.612878
454.710775	49.672033	73.617882
453.697801	56.309017	73.622887
453.064675	45.656388	73.627892
452.213351	46.120371	73.632897
452.130965	50.805884	73.637902
451.021892	45.572137	73.642906
450.270566	55.406068	73.647911
449.794451	48.179883	73.652916
449.137810	54.233993	73.657921
448.731636	47.803014	73.662926
447.631756	52.755253	73.667930
446.814201	55.393456	73.672935
446.539246	50.834221	73.677940
445.858771	58.503639	73.682945
445.398221	60.622401	73.687950
444.468910	55.205092	73.692954
443.297821	57.476799	73.697959
443.103586	50.707149	73.702964
442.503854	53.092116	73.707969
442.334993	52.186723	73.712974
441.426068	44.803014	73.717978
440.304749	56.139871	73.722983
439.877808	43.479528	73.727988
439.710804	57.264668	73.732993
438.598865	49.750362	73.737998
437.436854	37.524658	73.743002
436.803258	54.163799	73.748007
436.404711	35.899583	73.753012
436.304765	47.295469	73.758017
435.870752	50.181743	73.763022
434.960917	43.424208	73.768026
434.196291	54.570078	73.773031
433.645623	49.924680	73.778036
432.345058	57.289860	73.783041
431.911119	48.199322	73.788046
431.545744	43.582959	73.793050
430.816062	49.803129	73.798055
430.095887	40.821250	73.803060
428.741955	56.527584	73.808065
428.008569	53.287892	73.813070
427.848594	46.004773	73.818074
427.227581	53.261786	73.823079
427.178779	45.604373	73.828084
426.266831	48.218888	73.833089
424.872466	44.968924	73.838094
424.516464	43.188947	73.843098
423.802019	50.926943	73.848103
423.459724	47.806142	73.853108
423.218579	47.616912	73.858113
421.917588	40.975753	73.863118
421.373361	49.904638	73.868122
420.703314	46.895265	73.873127
420.385909	47.324200	73.878132
419.192425	53.755294	73.883137
418.584575	53.634038	73.888142
417.864057	45.248236	73.893146
417.080271	50.062237	73.898151
417.146261	56.127503	73.903156
416.417260	55.306657	73.908161
415.248558	42.528715	73.913166
414.432648	45.309525	73.918170
413.787632	48.716274	73.923175
413.884041	55.882314	73.928180
413.451593	50.381051	73.933185
412.325623	45.117449	73.938190
411.842952	47.018174	73.943194
410.873315	54.175469	73.948199
409.787669	39.684450	73.953204
409.194938	47.202257	73.958209
408.865743	50.117935	73.963214
408.398368	49.724727	73.968218
407.510914	50.524101	73.973223
406.829624	50.666471	73.978228
405.824382	53.548805	73.983233
405.316215	46.918614	73.988238
404.911874	49.423642	73.993242
404.195377	46.908124	73.998247
403.748299	35.521435	74.003252
402.831370	53.410242	74.008257
402.145028	47.431471	74.013262
402.125977	47.193918	74.018266
400.916371	49.509732	74.023271
400.179973	38.330904	74.028276
399.371454	47.354815	74.033281
398.827529	43.731366	74.038286
398.668782	41.208681	74.043290
397.727990	50.353151	74.048295
396.933279	42.965670	74.053300
396.334609	49.436927	74.058305
395.649675	49.066400	74.063310
395.137998	44.109215	74.068314
394.003483	47.957859	74.073319
393.719857	33.391375	74.078324
392.679131	50.991546	74.083329
392.222078	42.406267	74.088334
391.859787	33.563978	74.093338
391.099637	52.012459	74.098343
390.742580	38.132331	74.103348
389.572299	46.784450	74.108353
389.223058	41.772194	74.113358
388.162012	41.248638	74.118362
386.830838	46.070404	74.123367
386.394594	39.841948	74.128372
386.174282	40.903548	74.133377
385.904979	45.902127	74.138382
385.864193	38.315975	74.143386
384.880566	49.073085	74.148391
384.049699	41.990207	74.153396
383.146849	50.576762	74.158401
382.489019	43.241611	74.163406
381.783885	39.698686	74.168410
380.727189	50.947896	74.173415
379.913503	38.566997	74.178420
379.756649	47.646191	74.183425
379.151167	47.192975	74.188430
379.214567	41.592137	74.193434
377.886027	50.389797	74.198439
376.913145	45.896501	74.203444
376.443719	56.120650	74.208449
375.939223	41.971729	74.213454
375.455706	33.271396	74.218458
374.201252	47.167102	74.223463
374.023848	42.617605	74.228468
373.569397	37.065259	74.233473
372.194063	45.895803	74.238478
371.586281	41.425986	74.243482
370.859815	55.025172	74.248487
370.621778	43.335043	74.253492
369.994244	50.025183	74.258497
369.312414	44.304973	74.263502
368.444247	44.746201	74.268506
367.661253	53.828897	74.273511
367.516796	44.943353	74.278516
366.783650	46.544002	74.283521
365.792869	48.403136	74.288526
364.615628	35.276177	74.293530
363.979878	49.312942	74.298535
363.721124	43.833233	74.303540
363.255127	49.718103	74.308545
362.904510	45.586296	74.313550
362.609256	40.210732	74.318554
361.236072	48.643041	74.323559
361.002798	42.433088	74.328564
360.404092	47.057490	74.333569
359.422207	51.378506	74.338574
358.457427	44.071494	74.343578
357.499299	46.912605	74.348583
357.466501	45.848906	74.353588
356.930973	41.416047	74.358593
356.264566	51.559092	74.363598
355.545619	41.666022	74.368602
354.473410	46.652216	74.373607
354.007418	47.592118	74.378612
353.066934	40.585664	74.383617
352.161907	43.724367	74.388622
351.507905	41.517866	74.393626
351.041477	45.056240	74.398631
351.278297	41.917506	74.403636
350.738700	46.886230	74.408641
349.683207	49.856918	74.413646
348.838028	37.437613	74.418650
347.827623	44.954378	74.423655
347.526205	38.850838	74.428660
346.637213	38.918294	74.433665
345.718958	54.128017	74.438670
345.548591	46.180018	74.443674
344.510952	48.299803	74.448679
344.371279	47.117060	74.453684
343.858665	45.250254	74.458689
342.922705	43.506132	74.463694
342.419491	46.497029	74.468698
341.435529	46.094870	74.473703
340.600934	40.483740	74.478708
339.601001	42.795208	74.483713
338.974184	41.346242	74.488718
338.771743	42.215714	74.493722
337.938535	53.292819	74.498727
337.779870	49.447438	74.503732
337.412784	48.205388	74.508737
336.218700	46.289205	74.513742
335.755796	39.093937	74.518746
334.961372	47.905844	74.523751
334.557175	46.745940	74.528756
333.601380	43.202565	74.533761
332.765851	40.828244	74.538766
332.755288	41.860214	74.543770
331.010833	46.028526	74.548775
330.352906	44.914082	74.553780
330.199528	52.481718	74.558785
329.366146	44.952469	74.563790
329.329275	43.971569	74.568794
328.453331	48.635594	74.573799
327.610914	46.466915	74.578804
326.899564	47.061658	74.583809
326.249616	53.134365	74.588814
325.748595	44.692415	74.593818
324.868666	45.795233	74.598823
324.100927	46.335697	74.603828
323.277570	43.395641	74.608833
322.920832	48.980356	74.613838
322.990032	49.162653	74.618842
321.738561	51.083842	74.623847
320.768619	49.188453	74.628852
319.889460	47.877864	74.633857
319.516564	45.869884	74.638862
319.370785	52.365361	74.643866
318.398239	58.766503	74.648871
318.079774	52.258934	74.653876
316.955705	49.217664	74.658881
316.314927	53.323128	74.663886
315.943792	52.990009	74.668890
314.897933	51.306963	74.673895
314.091608	42.999444	74.678900
313.967660	50.273104	74.683905
313.427292	47.279020	74.688910
313.090661	42.161197	74.693914
311.742355	46.531997	74.698919
311.266286	46.068451	74.703924
310.390250	49.884652	74.708929
308.702341	53.896053	74.713934
308.805692	50.290354	74.718938
308.256401	53.141135	74.723943
307.459896	48.290014	74.728948
307.484533	48.927553	74.733953
307.205253	40.348530	74.738958
306.787607	40.894516	74.743962
305.130635	54.391491	74.748967
304.621677	47.000052	74.753972
303.449050	42.268659	74.758977
302.411581	50.764617	74.763982
302.378941	51.082388	74.768986
301.703101	47.436566	74.773991
301.386754	41.295330	74.778996
300.968389	35.413145	74.784001
299.827072	41.830579	74.789006
298.956624	36.946351	74.794010
298.369594	45.694294	74.799015
298.120309	47.190311	74.804020
297.481953	49.334427	74.809025
296.897327	43.860056	74.814030
295.764210	47.839130	74.819034
294.329503	51.790560	74.824039
294.194046	38.987142	74.829044
293.756376	42.653213	74.834049
293.605297	45.821375	74.839054
293.042373	40.366180	74.844058
291.643540	40.364726	74.849063
291.100519	39.571232	74.854068
290.949230	39.050838	74.859073
290.167954	40.598566	74.864078
289.224119	29.727682	74.869082
288.449073	42.378795	74.874087
288.285233	37.942239	74.879092
287.715808	43.326184	74.884097
286.452951	42.352141	74.889102
286.020550	34.854437	74.894106
285.334009	46.716747	74.899111
285.091556	40.937825	74.904116
283.881740	47.682775	74.909121
282.627179	43.001746	74.914126
282.543933	39.803799	74.919130
282.227457	44.657314	74.924135
281.955942	42.659197	74.929140
280.749927	51.858612	74.934145
279.582434	43.442095	74.939150
279.046354	37.963356	74.944154
278.594588	46.362872	74.949159
278.415410	40.800460	74.954164
277.550413	45.462220	74.959169
276.317654	50.640148	74.964174
276.109626	40.678079	74.969178
275.354083	52.573930	74.974183
275.049150	41.722999	74.979188
274.160679	47.654628	74.984193
273.216222	43.312794	74.989198
272.783180	38.440831	74.994202
272.119617	45.717378	74.999207
271.992676	39.606441	75.004212
270.846419	48.502341	75.009217
269.699169	43.836867	75.014222
269.533358	42.894647	75.019226
269.112872	49.485361	75.024231
268.199112	49.994418	75.029236
267.320911	51.324305	75.034241
266.460395	52.166848	75.039246
266.218842	47.630723	75.044250
265.995757	52.000104	75.049255
265.053989	40.764150	75.054260
264.050582	45.946580	75.059265
263.045689	48.579421	75.064270
263.071371	38.643214	75.069274
262.231437	44.096421	75.074279
261.738940	42.427086	75.079284
260.390053	42.184200	75.084289
259.999126	43.472800	75.089294
259.755518	39.337664	75.094298
258.983489	43.282087	75.099303
258.611962	47.576653	75.104308
257.610341	34.715275	75.109313
256.550540	45.384799	75.114318
256.474273	39.168868	75.119322
256.191785	49.527538	75.124327
255.273227	45.221135	75.129332
254.274449	34.656105	75.134337
253.535852	45.556345	75.139342
253.322823	45.297967	75.144346
251.913744	49.113970	75.149351
251.341793	40.383818	75.154356
250.961545	37.870690	75.159361
250.137110	47.350865	75.164366
249.804014	41.073173	75.169370
248.802461	40.051193	75.174375
248.178337	41.111362	75.179380
247.743009	36.269398	75.184385
247.040657	38.959323	75.189390
246.937023	35.567517	75.194394
245.551584	54.637880	75.199399
244.725916	42.933637	75.204404
244.490062	45.203360	75.209409
243.828694	42.581322	75.214414
243.548053	34.778551	75.219418
242.040984	43.345534	75.224423
241.513245	44.005916	75.229428
241.130838	43.673551	75.234433
240.560702	51.971789	75.239438
239.737760	45.633201	75.244442
238.632443	44.130882	75.249447
238.367365	39.699840	75.254452
237.696344	45.004499	75.259457
237.178418	54.228863	75.264462
236.811297	37.485276	75.269466
235.337879	47.427593	75.274471
234.725163	37.689628	75.279476
234.598074	42.106494	75.284481
233.531677	46.144008	75.289486
233.601869	37.231954	75.294490
232.957063	50.789510	75.299495
231.888888	39.255913	75.304500
231.318432	38.462787	75.309505
230.877145	42.234870	75.314510
230.061576	37.462428	75.319514
229.051384	45.373095	75.324519
228.521340	46.058740	75.329524
227.946931	43.094583	75.334529
227.016298	50.094434	75.339534
226.360471	42.706872	75.344538
225.556033	49.160518	75.349543
225.539520	48.634786	75.354548
225.153307	53.160806	75.359553
223.864225	42.581204	75.364558
223.110892	44.575705	75.369562
222.372116	51.936198	75.374567
221.856328	46.444120	75.379572
221.502519	52.391472	75.384577
220.297026	47.160899	75.389582
219.726673	43.382939	75.394586
219.030186	49.543362	75.399591
219.023425	43.219998	75.404596
218.168386	48.311086	75.409601
217.149469	44.053473	75.414606
216.435268	43.718778	75.419610
215.260589	48.289956	75.424615
214.972217	46.017645	75.429620
214.884122	42.841058	75.434625
214.352125	43.023386	75.439630
213.577018	33.018020	75.444634
212.645099	45.771024	75.449639
212.165482	46.443685	75.454644
211.965783	44.823239	75.459649
210.634360	44.035039	75.464654
209.956218	43.295898	75.469658
209.307328	41.206564	75.474663
208.881686	45.727499	75.479668
207.917075	49.052087	75.484673
207.175776	46.544014	75.489678
206.529684	32.215352	75.494682
206.087021	46.022051	75.499687
205.746431	35.515123	75.504692
204.954556	44.081089	75.509697
203.531279	49.161040	75.514702
203.376327	44.206286	75.519706
202.514368	46.750693	75.524711
202.134202	43.794688	75.529716
201.993400	45.137516	75.534721
200.877649	46.823510	75.539726
200.198575	37.934903	75.544730
199.336721	41.947622	75.549735
198.969131	43.995995	75.554740
198.342795	50.440429	75.559745
197.336887	44.604108	75.564750
196.795928	38.085757	75.569754
196.376473	46.263432	75.574759
195.581983	43.945258	75.579764
194.826140	40.630126	75.584769
193.801372	48.811308	75.589774
193.807163	46.397790	75.594778
193.250199	47.314224	75.599783
191.952231	54.246399	75.604788
191.515000	40.961865	75.609793
190.921110	48.943668	75.614798
190.409841	40.273781	75.619802
189.267952	40.154106	75.624807
188.256717	44.713455	75.629812
187.834309	40.563978	75.634817
187.238388	50.038537	75.639822
187.315759	48.177187	75.644826
186.475643	50.129337	75.649831
185.946279	47.736112	75.654836
184.889096	35.860409	75.659841
184.145041	46.975127	75.664846
184.176203	40.424621	75.669850
183.154316	49.947333	75.674855
182.129025	45.078622	75.679860
181.540258	51.758181	75.684865
180.754512	54.088620	75.689870
180.862738	50.517611	75.694874
179.779605	51.556216	75.699879
178.277428	53.706722	75.704884
177.885206	44.892883	75.709889
177.104436	50.127552	75.714894
176.957152	48.658376	75.719898
176.727812	53.058038	75.724903
176.002435	48.428424	75.729908
175.271871	43.969822	75.734913
174.519632	48.630819	75.739918
173.710500	30.660476	75.744922
172.955314	49.737660	75.749927
172.090273	46.601503	75.754932
171.467962	48.054504	75.759937
170.248922	55.701793	75.764942
170.211080	39.895267	75.769946
169.951080	52.292715	75.774951
169.641717	56.293621	75.779956
169.015393	52.941290	75.784961
167.683900	57.566992	75.789966
167.437802	49.709359	75.794970
166.809463	52.467130	75.799975
165.506316	56.806543	75.804980
165.314233	50.298646	75.809985
164.449147	55.624742	75.814990
163.993440	50.564056	75.819994
162.328070	52.225864	75.824999
161.599658	53.088408	75.830004
161.662946	42.735261	75.835009
160.934732	53.238623	75.840014
160.776261	38.928214	75.845018
160.142836	43.979344	75.850023
159.725385	42.360706	75.855028
158.726085	43.682162	75.860033
157.935397	49.327850	75.865038
157.151178	59.765032	75.870042
156.683498	57.808840	75.875047
155.498170	56.205001	75.880052
155.129392	48.012765	75.885057
154.412997	55.395085	75.890062
154.172214	43.999921	75.895066
153.604827	51.444716	75.900071
152.339095	47.486782	75.905076
152.066314	43.388628	75.910081
151.084729	51.753060	75.915086
150.609941	47.128648	75.920090
149.707687	41.566265	75.925095
148.670330	49.670669	75.930100
148.320114	42.222840	75.935105
147.838067	54.859263	75.940110
147.438084	47.013015	75.945114
147.188750	46.345629	75.950119
146.337832	45.405605	75.955124
145.138939	48.116722	75.960129
144.543648	38.426709	75.965134
144.151910	35.407174	75.970138
143.221213	52.477339	75.975143
142.478033	50.033938	75.980148
141.965249	44.679903	75.985153
141.270517	47.848506	75.990158
141.328697	50.834752	75.995162
140.179170	47.551989	76.000167
139.337019	51.330830	76.005172
139.070689	41.976765	76.010177
137.932437	47.916103	76.015182
136.930379	46.074417	76.020186
136.328403	52.004316	76.025191
135.664798	48.750745	76.030196
135.485303	47.260648	76.035201
134.990556	50.987827	76.040206
134.647838	34.946226	76.045210
133.467763	41.318626	76.050215
132.463501	53.110682	76.055220
132.094571	36.409273	76.060225
131.602523	44.394537	76.065230
131.061021	43.659614	76.070234
130.453662	51.367431	76.075239
129.800476	46.943727	76.080244
128.976211	44.049259	76.085249
127.737363	47.064843	76.090254
127.211383	41.899773	76.095258
126.642007	45.762106	76.100263
126.335063	47.015004	76.105268
126.215079	40.623826	76.110273
124.499763	48.641970	76.115278
123.935937	46.030861	76.120282
123.412582	49.084829	76.125287
122.907355	48.551702	76.130292
122.594230	46.040105	76.135297
120.934534	46.116579	76.140302
120.786494	41.537993	76.145306
119.924818	48.762862	76.150311
119.618153	44.323568	76.155316
119.337363	46.509424	76.160321
118.254177	47.409507	76.165326
117.678377	43.742623	76.170330
117.223041	53.851070	76.175335
116.443109	47.333044	76.180340
115.387173	43.025360	76.185345
114.445400	56.919602	76.190350
114.215375	43.251426	76.195354
113.819629	46.089713	76.200359
113.224618	52.324322	76.205364
112.579347	46.102140	76.210369
111.475940	53.348717	76.215374
111.254804	40.800003	76.220378
110.376708	47.818490	76.225383
109.170573	43.611158	76.230388
108.869300	46.733231	76.235393
108.144576	52.282359	76.240398
107.931238	46.353210	76.245402
107.237822	49.336077	76.250407
106.193626	50.399600	76.255412
105.888339	37.821108	76.260417
104.989876	45.614748	76.265422
104.599570	42.164735	76.270426
103.118684	52.617147	76.275431
102.297852	47.919444	76.280436
101.687845	52.901440	76.285441
101.745244	50.961020	76.290446
101.180303	46.946113	76.295450
100.590563	51.829114	76.300455
100.130965	47.953243	76.305460
99.400535	44.097359	76.310465
98.316476	51.796908	76.315470
98.001554	47.109179	76.320474
97.444369	48.826138	76.325479
96.092301	40.594872	76.330484
95.257438	42.626656	76.335489
94.342912	54.334257	76.340494
94.231528	48.087254	76.345498
94.177058	54.299848	76.350503
93.591354	51.341594	76.355508
92.691741	47.996658	76.360513
91.979376	52.065472	76.365518
91.508440	44.736236	76.370522
90.441442	45.245154	76.375527
89.540765	47.382953	76.380532
89.096393	40.348752	76.385537
88.139267	48.559796	76.390542
87.905129	44.543438	76.395546
87.390520	48.930431	76.400551
86.854167	47.172721	76.405556
85.930718	39.782920	76.410561
84.788430	52.365568	76.415566
84.755645	38.704637	76.420570
83.926938	46.072268	76.425575
82.830192	47.666614	76.430580
82.490189	47.379490	76.435585
81.485592	45.545357	76.440590
81.609952	39.063744	76.445594
81.035826	46.183268	76.450599
79.792314	47.331491	76.455604
79.385167	44.172902	76.460609
78.688445	48.012469	76.465614
78.499272	43.653293	76.470618
76.920467	50.131959	76.475623
76.009037	50.886165	76.480628
75.981629	43.018685	76.485633
74.805714	41.768497	76.490638
74.954660	45.127968	76.495642
74.111557	51.468662	76.500647
72.936934	48.762159	76.505652
72.400011	47.775026	76.510657
71.597668	54.214121	76.515662
71.575100	40.455524	76.520666
71.378331	42.653027	76.525671
69.929208	48.501210	76.530676
69.245751	48.159293	76.535681
68.418049	55.556756	76.540686
68.194689	50.470460	76.545690
67.795537	43.247731	76.550695
66.524158	51.040580	76.555700
66.003503	48.024208	76.560705
65.336743	50.600298	76.565710
64.857256	43.042812	76.570714
63.965777	46.983662	76.575719
63.173153	52.852705	76.580724
62.679385	53.165067	76.585729
61.908649	61.121152	76.590734
61.491943	50.562558	76.595738
61.244965	50.838135	76.600743
59.877147	49.121146	76.605748
59.282167	47.098772	76.610753
58.636574	49.519664	76.615758
58.418557	47.249515	76.620762
57.628224	55.932464	76.625767
56.333733	58.811168	76.630772
56.149640	44.069010	76.635777
55.279928	48.737926	76.640782
55.424567	44.821226	76.645786
54.158465	40.911543	76.650791
53.257175	45.065247	76.655796
52.689315	51.481113	76.660801
52.372777	52.412391	76.665806
51.802819	45.032644	76.670810
50.491262	46.123466	76.675815
49.682072	49.794832	76.680820
49.430614	42.627700	76.685825
49.113445	50.289714	76.690830
48.788350	47.057064	76.695834
47.896960	50.988823	76.700839
46.921095	46.611380	76.705844
46.700475	39.016621	76.710849
45.528989	44.653402	76.715854
44.734858	40.919760	76.720858
43.841712	43.218896	76.725863
43.419844	49.359090	76.730868
42.903379	41.700587	76.735873
42.579424	43.004955	76.740878
41.595879	47.587212	76.745882
40.872913	47.693756	76.750887
40.195919	51.026293	76.755892
39.705958	44.229244	76.760897
38.713300	50.629527	76.765902
38.140017	48.838290	76.770906
37.356398	47.167584	76.775911
36.869252	42.523996	76.780916
36.704048	37.956255	76.785921
35.928588	48.919270	76.790926
34.981357	50.589038	76.795930
34.327751	49.433639	76.800935
33.676642	60.674928	76.805940
33.427934	41.849901	76.810945
32.512442	47.504764	76.815950
31.741578	43.523597	76.820954
31.001462	33.641748	76.825959
30.241952	46.742547	76.830964
30.052970	45.219348	76.835969
28.927683	41.247637	76.840974
28.603646	38.392154	76.845978
28.032293	40.932944	76.850983
26.934821	44.805308	76.855988
25.940322	38.732228	76.860993
25.031015	43.564240	76.865998
24.915349	44.995124	76.871002
24.416381	49.507326	76.876007
23.737303	44.405231	76.881012
23.947834	35.905290	76.886017
22.586611	51.069003	76.891022
22.057423	36.839157	76.896026
21.157470	41.143021	76.901031
20.076350	47.210732	76.906036
19.291508	44.314659	76.911041
18.574827	55.699416	76.916046
18.349253	46.540079	76.921050
18.069455	41.865284	76.926055
17.312363	45.302340	76.931060
17.181639	46.495821	76.936065
16.229783	51.326449	76.941070
15.735632	44.093571	76.946074
14.882114	47.593342	76.951079
13.268387	59.659242	76.956084
12.789661	47.325617	76.961089
11.976064	52.017285	76.966094
11.692457	51.527482	76.971098
11.194121	48.575181	76.976103
10.830525	49.338489	76.981108
10.485099	44.671395	76.986113
9.487636	45.953884	76.991118
8.946743	41.673967	76.996122
7.844140	44.216642	77.001127
6.521481	50.144993	77.006132
6.223395	33.493838	77.011137
5.535416	49.192997	77.016142
5.452102	45.984024	77.021147
5.221994	51.887274	77.026151
4.339981	46.596176	77.031156
3.318963	33.500205	77.036161