Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
PM-HIP_00000.hld	3462.476549	445330.573305	7984.536742	317110579.293257	3537.435449	3504.307144	397.263978	1.404338	0.000000	2904.350148	10.756905	-134.713000	-46.491500	0.391817
PM-HIP_00001.hld	3465.513396	446895.844368	8627.565715	317653647.496064	3537.393852	3504.362348	428.890257	1.406865	0.000000	2117.363976	26.776753	-134.664000	-46.491500	0.146651
PM-HIP_00002.hld	3466.252875	446283.310926	8812.628998	317785955.147489	3534.404505	3504.233878	437.998846	1.404352	0.000000	2843.165559	13.053927	-134.614000	-46.491500	0.049138
PM-HIP_00003.hld	3468.548497	437544.299532	9082.374522	318196860.964906	3534.098597	3504.679822	451.113983	1.375074	0.000000	1930.400827	32.678272	-134.564000	-46.491500	-0.025735
PM-HIP_00004.hld	3468.170588	441269.826808	9138.793696	318129199.017913	3535.112488	3504.384598	453.964545	1.387077	0.000000	0.000100	72.576562	-134.514000	-46.491500	0.017623
PM-HIP_00005.hld	3469.388174	450224.434119	9653.318803	318347224.774767	3534.658476	3504.367680	479.359064	1.414256	0.000000	2303.382342	25.750478	-134.714000	-46.441500	-0.019604
PM-HIP_00006.hld	3466.243523	454012.644821	8696.991755	317784281.670526	3538.237105	3505.396082	432.252666	1.428682	0.000000	2069.856558	27.498960	-134.664000	-46.441500	-0.016471
PM-HIP_00007.hld	3470.395816	426807.255061	9413.616390	318527712.903566	3533.261670	3504.400329	467.323600	1.339938	0.000000	0.000100	77.292687	-134.614000	-46.441500	-0.023929
PM-HIP_00008.hld	3469.638049	394220.244863	8508.198162	318391977.597004	3534.091815	3504.388672	422.465615	1.238160	0.000000	968.214534	54.736591	-134.564000	-46.441500	-0.005990
PM-HIP_00009.hld	3465.587027	447714.223342	8768.760647	317666820.251918	3533.011221	3503.880428	435.900248	1.409383	0.000000	0.000100	68.625669	-134.514000	-46.441500	-0.039227
PM-HIP_00010.hld	3469.586540	432126.639048	9074.725840	318382752.037264	3534.530130	3505.300565	450.602478	1.357255	0.000000	0.000100	73.611849	-134.714000	-46.391500	0.007479
PM-HIP_00011.hld	3466.386627	473602.688797	9388.625710	317809888.796203	3531.460358	3504.219854	466.609043	1.490208	0.000000	442.646440	60.692153	-134.664000	-46.391500	0.001378
PM-HIP_00012.hld	3466.748071	449824.049612	8868.501492	317874570.831316	3534.600585	3504.789226	440.714336	1.415099	0.000000	2815.379200	13.592056	-134.614000	-46.391500	-0.014178
PM-HIP_00013.hld	3468.049734	439068.781892	9018.163266	318107562.491203	3533.451968	3504.565106	447.987530	1.380253	0.000000	0.000100	71.981295	-134.564000	-46.391500	-0.001783
PM-HIP_00014.hld	3472.536358	374288.222875	8870.548758	318911292.481703	3536.354758	3504.182220	440.098985	1.173644	0.000000	0.000100	83.048347	-134.514000	-46.391500	-0.001879
PM-HIP_00015.hld	3464.413799	473205.805285	8757.796157	317456957.732340	3533.396666	3504.938190	435.499074	1.490614	0.000000	0.000100	64.867195	-134.714000	-46.341500	-0.015130
PM-HIP_00016.hld	3468.555324	456059.790073	9437.111954	318198083.330484	3534.960058	3504.799976	468.732596	1.433258	0.000000	0.000100	72.523800	-134.664000	-46.341500	-0.016513
PM-HIP_00017.hld	3468.443994	441507.533199	8968.776471	318178149.803791	3533.430171	3505.364376	445.484761	1.387611	0.000000	0.000100	71.207910	-134.614000	-46.341500	-0.009953
PM-HIP_00018.hld	3467.332931	445018.315001	8973.376499	317979247.587825	3534.796514	3504.527819	445.852627	1.399520	0.000000	0.000100	70.665511	-134.564000	-46.341500	0.009866
PM-HIP_00019.hld	3463.873252	483184.397249	8827.433200	317360289.694265	3533.847714	3504.925763	439.028765	1.522511	0.000000	2878.031869	11.452903	-134.514000	-46.341500	0.029783
PM-HIP_00020.hld	3466.403640	460754.113832	9018.597349	317812933.296913	3533.387075	3504.720639	448.216709	1.449765	0.000000	0.000100	68.599851	-134.714000	-46.291500	-0.013437
PM-HIP_00021.hld	3467.256996	455134.342791	9095.271083	317965655.879410	3533.968397	3504.787571	451.918759	1.431395	0.000000	1118.924855	47.678380	-134.664000	-46.291500	-0.004230
PM-HIP_00022.hld	3468.989942	459190.229934	9632.321759	318275907.609400	3533.537202	3504.743800	478.369990	1.442743	0.000000	0.000100	73.518156	-134.614000	-46.291500	0.041360
PM-HIP_00023.hld	3466.284861	481221.500334	9264.731366	317791678.633684	3535.892592	3505.240780	460.464761	1.514267	0.000000	0.000100	67.484751	-134.564000	-46.291500	-0.001708
PM-HIP_00024.hld	3466.998061	467557.836531	9433.468929	317919311.317520	3534.663457	3504.170853	468.757034	1.470681	0.000000	2672.752397	16.774738	-134.514000	-46.291500	0.014576