Thu Jun 16 18:01:39 2022

Number of Points = 9930

Depth (nm)	Load (N)	Time (s)
-0.884626	86.185123	0.000000
-1.200800	87.977375	0.005005
-0.737930	82.314660	0.010010
-0.880113	100.069091	0.015014
-1.058269	85.516314	0.020019
-1.234031	66.060626	0.025024
-1.834994	64.339432	0.030029
-1.482822	55.967469	0.035034
-2.153985	52.416952	0.040038
-2.484674	35.673216	0.045043
-2.315448	31.928973	0.050048
-2.898751	21.967084	0.055053
-3.030400	10.358975	0.060058
-3.598910	12.775185	0.065062
-3.470006	13.632315	0.070067
-3.902536	-4.231065	0.075072
-4.185398	3.587789	0.080077
-3.978798	-16.891099	0.085082
-4.964740	-18.389039	0.090086
-4.870705	-22.786276	0.095091
-5.153308	-29.080080	0.100096
-5.577619	-19.177143	0.105101
-6.061571	-33.801112	0.110106
-6.149840	-35.494256	0.115110
-6.612279	-38.029942	0.120115
-7.018206	-42.252408	0.125120
-7.331756	-36.438711	0.130125
-7.380489	-23.672110	0.135130
-7.517352	-27.694280	0.140134
-7.446418	-33.474894	0.145139
-7.652723	-42.706539	0.150144
-8.292256	-22.654651	0.155149
-8.773665	-28.672415	0.160154
-9.084474	-34.667265	0.165158
-9.121634	-20.605450	0.170163
-9.021396	-33.447948	0.175168
-9.181587	-28.610236	0.180173
-9.611727	-26.774303	0.185178
-10.078572	-37.301654	0.190182
-10.842553	-35.801229	0.195187
-10.443800	-39.460854	0.200192
-10.773656	-32.547607	0.205197
-10.686689	-38.369640	0.210202
-11.229067	-35.294987	0.215206
-11.981253	-27.084176	0.220211
-12.028503	-35.072806	0.225216
-12.805329	-27.181513	0.230221
-12.141351	-43.037273	0.235226
-12.353018	-36.475930	0.240230
-12.532454	-33.112013	0.245235
-12.527620	-37.358261	0.250240
-13.159963	-35.193539	0.255245
-13.466683	-33.647923	0.260250
-13.573618	-23.647382	0.265254
-13.914071	-36.413302	0.270259
-14.297827	-34.308601	0.275264
-15.490614	-27.083257	0.280269
-15.366976	-28.152893	0.285274
-15.515176	-37.646800	0.290278
-14.947428	-24.198160	0.295283
-15.289873	-27.557721	0.300288
-15.827281	-28.799975	0.305293
-15.671108	-37.680228	0.310298
-16.211812	-32.331246	0.315302
-16.850214	-36.282764	0.320307
-16.798856	-30.599511	0.325312
-17.022303	-16.074304	0.330317
-16.742266	-32.957560	0.335322
-17.522316	-20.148634	0.340326
-18.026148	-32.042866	0.345331
-18.304710	-26.235046	0.350336
-18.652915	-28.197084	0.355341
-18.948528	-29.103418	0.360346
-18.805103	-33.031714	0.365350
-18.687332	-27.771126	0.370355
-18.441535	-29.478731	0.375360
-19.636754	-34.480566	0.380365
-19.906358	-37.773632	0.385370
-20.402127	-24.534787	0.390374
-20.343778	-26.893225	0.395379
-19.866749	-36.537317	0.400384
-20.752485	-32.710595	0.405389
-21.542034	-42.499349	0.410394
-21.543160	-31.651485	0.415398
-21.834715	-27.849949	0.420403
-21.569341	-28.271360	0.425408
-21.666103	-31.763862	0.430413
-22.107128	-37.000923	0.435418
-22.867439	-30.447073	0.440422
-23.215622	-23.173660	0.445427
-23.283060	-25.779162	0.450432
-23.813246	-24.841233	0.455437
-23.655750	-27.119768	0.460442
-23.604771	-34.587844	0.465446
-23.697458	-31.167329	0.470451
-24.035063	-27.472229	0.475456
-24.678211	-26.421811	0.480461
-25.138535	-20.596184	0.485466
-25.219247	-25.427335	0.490470
-25.717957	-22.389295	0.495475
-25.526431	-31.873443	0.500480
-25.541606	-19.526051	0.505485
-25.998581	-36.641384	0.510490
-26.525927	-26.270273	0.515494
-26.407074	-34.463438	0.520499
-26.507624	-30.296478	0.525504
-26.934141	-32.925410	0.530509
-27.407412	-29.492019	0.535514
-28.080126	-34.044499	0.540518
-27.975312	-34.688975	0.545523
-27.942434	-23.986915	0.550528
-28.040987	-23.481988	0.555533
-27.892187	-39.077105	0.560538
-28.860119	-38.609441	0.565542
-29.413061	-33.798675	0.570547
-29.476886	-20.814611	0.575552
-29.669986	-16.503705	0.580557
-29.579358	-39.692802	0.585562
-30.060027	-40.357429	0.590566
-30.888373	-36.925541	0.595571
-30.923015	-41.032276	0.600576
-31.330172	-32.132945	0.605581
-30.891243	-44.087466	0.610586
-30.701784	-27.154053	0.615590
-30.733192	-20.206561	0.620595
-31.788649	-30.375202	0.625600
-32.272662	-30.111223	0.630605
-32.004675	-41.857942	0.635610
-32.626893	-23.650129	0.640614
-32.962795	-30.166567	0.645619
-33.427478	-25.998919	0.650624
-34.108320	-27.452564	0.655629
-33.800671	-37.072609	0.660634
-33.897902	-26.121254	0.665638
-34.057335	-31.331846	0.670643
-34.063429	-31.785248	0.675648
-34.260969	-31.588835	0.680653
-34.513693	-36.171061	0.685658
-35.214699	-27.806912	0.690662
-35.805999	-29.942661	0.695667
-35.669488	-38.733833	0.700672
-36.303686	-27.881186	0.705677
-35.648645	-26.186604	0.710682
-35.813229	-28.057541	0.715686
-36.678418	-33.536158	0.720691
-37.288390	-32.900544	0.725696
-37.451200	-21.183435	0.730701
-37.548030	-25.513809	0.735706
-37.702458	-26.815702	0.740710
-37.232668	-20.140851	0.745715
-37.669006	-34.650544	0.750720
-38.803822	-19.600628	0.755725
-39.071858	-32.879585	0.760730
-39.245686	-30.311858	0.765734
-39.343994	-28.573282	0.770739
-39.143203	-36.483230	0.775744
-39.318674	-25.044707	0.780749
-39.221954	-31.305201	0.785754
-39.928753	-37.427378	0.790758
-40.408323	-26.309547	0.795763
-40.719291	-33.885225	0.800768
-40.851993	-18.961652	0.805773
-41.035018	-31.812386	0.810778
-42.159877	-35.961717	0.815782
-42.318228	-24.931103	0.820787
-41.616618	-30.971423	0.825792
-41.957299	-30.857607	0.830797
-42.153388	-34.441721	0.835802
-42.605122	-40.919872	0.840806
-42.833461	-42.544484	0.845811
-42.709515	-41.558681	0.850816
-43.808017	-27.553124	0.855821
-44.095199	-38.294250	0.860826
-44.140686	-35.856846	0.865830
-44.287141	-21.150314	0.870835
-44.079824	-30.980986	0.875840
-44.648014	-30.112740	0.880845
-44.603078	-32.262079	0.885850
-45.426763	-39.293978	0.890854
-46.279924	-22.717647	0.895859
-45.901556	-25.611792	0.900864
-46.024161	-27.896128	0.905869
-46.022119	-40.036928	0.910874
-45.877797	-36.106269	0.915878
-46.196866	-26.287126	0.920883
-46.440622	-28.157212	0.925888
-47.220923	-28.796984	0.930893
-47.456457	-33.549963	0.935898
-47.786576	-36.019216	0.940902
-47.488193	-28.766137	0.945907
-48.060476	-29.337389	0.950912
-49.050840	-26.610253	0.955917
-49.057927	-30.662646	0.960922
-49.203871	-21.511202	0.965926
-49.305836	-24.751666	0.970931
-49.106070	-38.145810	0.975936
-49.569656	-32.061960	0.980941
-49.417399	-28.033659	0.985946
-50.243690	-34.590792	0.990950
-50.671722	-27.492322	0.995955
-50.640650	-25.868653	1.000960
-50.957051	-28.373322	1.005965
-51.101300	-29.763910	1.010970
-51.128764	-28.147734	1.015974
-51.548651	-37.534978	1.020979
-52.200817	-27.765265	1.025984
-52.532653	-24.748487	1.030989
-52.251889	-42.180769	1.035994
-52.314570	-33.151120	1.040998
-52.451214	-26.918068	1.046003
-52.979894	-36.735920	1.051008
-53.830686	-26.243087	1.056013
-54.132892	-24.403531	1.061018
-53.388185	-32.005688	1.066022
-53.720245	-32.155128	1.071027
-54.020904	-39.041325	1.076032
-54.799564	-32.862984	1.081037
-54.906890	-30.846485	1.086042
-54.799299	-28.385839	1.091046
-55.237983	-20.125908	1.096051
-55.924399	-27.994011	1.101056
-56.212746	-42.042666	1.106061
-56.414063	-32.575160	1.111066
-56.326709	-32.635571	1.116070
-56.520455	-22.514237	1.121075
-56.319772	-28.057914	1.126080
-57.355351	-28.854782	1.131085
-57.731721	-37.152068	1.136090
-58.341195	-42.258387	1.141094
-58.520205	-32.447498	1.146099
-58.215565	-30.874861	1.151104
-58.614138	-23.394330	1.156109
-58.386469	-34.734537	1.161114
-58.412791	-33.571774	1.166118
-58.574938	-29.847168	1.171123
-59.189162	-31.899412	1.176128
-59.699129	-24.733238	1.181133
-59.993422	-24.019862	1.186138
-59.925918	-26.869046	1.191142
-60.725190	-28.979400	1.196147
-60.805129	-22.190914	1.201152
-61.340576	-24.585884	1.206157
-61.605727	-35.162048	1.211162
-61.765230	-30.334811	1.216166
-61.603380	-28.734235	1.221171
-61.405780	-30.893019	1.226176
-61.650292	-23.605269	1.231181
-62.143203	-26.637284	1.236186
-63.012871	-19.378712	1.241190
-63.149758	-32.544279	1.246195
-63.016440	-34.296436	1.251200
-63.287967	-24.677922	1.256205
-63.250334	-24.384624	1.261210
-64.084014	-23.469836	1.266214
-64.315548	-17.016980	1.271219
-64.325364	-29.375928	1.276224
-64.685158	-27.350458	1.281229
-64.478848	-20.696391	1.286234
-65.254880	-31.188128	1.291238
-65.930041	-20.951224	1.296243
-66.199467	-33.333264	1.301248
-66.055628	-29.334650	1.306253
-66.075310	-35.039513	1.311258
-65.986624	-28.511823	1.316262
-66.373145	-18.527429	1.321267
-67.077539	-27.480533	1.326272
-67.603683	-28.945533	1.331277
-67.701818	-35.738230	1.336282
-67.946862	-33.694236	1.341286
-68.009858	-28.326136	1.346291
-67.810789	-33.358014	1.351296
-68.106871	-24.169330	1.356301
-68.021352	-27.201538	1.361306
-69.172756	-26.904804	1.366310
-69.528960	-29.664331	1.371315
-69.481269	-34.403638	1.376320
-69.887785	-27.608341	1.381325
-69.774156	-29.526340	1.386330
-70.375298	-21.986779	1.391334
-71.072236	-15.092772	1.396339
-71.087555	-26.450837	1.401344
-71.630716	-21.255248	1.406349
-71.571431	-28.246808	1.411354
-71.312843	-29.992241	1.416358
-71.467807	-21.501090	1.421363
-71.356556	-25.239782	1.426368
-71.721258	-25.007060	1.431373
-72.079688	-29.810266	1.436378
-72.789912	-32.762956	1.441382
-72.793503	-23.288463	1.446387
-72.927884	-30.348152	1.451392
-73.824971	-18.786917	1.456397
-74.171870	-26.697118	1.461402
-74.592030	-29.520954	1.466406
-74.783114	-21.168463	1.471411
-74.216997	-18.320308	1.476416
-74.302636	-15.647385	1.481421
-74.685274	-18.854783	1.486426
-74.628114	-30.284706	1.491430
-75.651490	-20.047968	1.496435
-75.711617	-20.298976	1.501440
-75.964444	-19.524084	1.506445
-76.027571	-34.370006	1.511450
-76.301483	-27.805182	1.516454
-76.977981	-21.855927	1.521459
-77.213954	-29.068612	1.526464
-77.488220	-18.136931	1.531469
-77.806179	-30.964274	1.536474
-77.491071	-37.650347	1.541478
-77.751967	-29.110518	1.546483
-77.671433	-25.872731	1.551488
-78.382126	-25.528371	1.556493
-79.063985	-27.712881	1.561498
-78.801624	-25.302872	1.566502
-79.268017	-28.240513	1.571507
-79.116423	-26.439748	1.576512
-79.500280	-17.255298	1.581517
-80.143521	-14.464178	1.586522
-80.272587	-24.145634	1.591526
-80.806579	-24.502913	1.596531
-81.022075	-33.702551	1.601536
-81.191680	-20.558651	1.606541
-81.179482	-23.841856	1.611546
-81.101250	-16.480669	1.616550
-81.791138	-21.795874	1.621555
-82.093562	-24.015271	1.626560
-82.629059	-21.764240	1.631565
-82.372809	-28.926173	1.636570
-82.288225	-29.913588	1.641574
-82.484868	-15.678031	1.646579
-83.329198	-23.680841	1.651584
-83.946362	-18.269099	1.656589
-83.884669	-24.132043	1.661594
-84.192515	-28.976065	1.666598
-84.180112	-21.405013	1.671603
-83.912603	-30.952819	1.676608
-84.307866	-25.843827	1.681613
-84.957192	-27.839854	1.686618
-85.625275	-20.872581	1.691622
-85.756365	-14.719269	1.696627
-85.572155	-31.083734	1.701632
-85.939612	-22.801343	1.706637
-86.282470	-37.115843	1.711642
-86.962973	-25.037541	1.716646
-87.495529	-20.200442	1.721651
-87.369554	-40.204645	1.726656
-87.505331	-22.800571	1.731661
-87.681763	-28.971426	1.736666
-87.585137	-35.768488	1.741670
-87.845747	-30.509794	1.746675
-87.414852	-35.616191	1.751680
-87.977633	-31.873321	1.756685
-88.311642	-39.491551	1.761690
-88.739570	-34.318167	1.766694
-89.299326	-20.798630	1.771699
-89.590271	-35.923582	1.776704
-90.203096	-26.204863	1.781709
-90.221654	-36.797900	1.786714
-90.399131	-31.490990	1.791718
-90.769590	-32.360088	1.796723
-90.302110	-26.879388	1.801728
-90.540786	-34.752221	1.806733
-90.790453	-24.055957	1.811738
-91.428669	-30.725064	1.816742
-91.960065	-19.332294	1.821747
-91.930940	-29.761359	1.826752
-92.538866	-24.262651	1.831757
-93.189636	-31.677985	1.836762
-93.013752	-25.231498	1.841766
-93.105400	-20.456316	1.846771
-93.480606	-17.952975	1.851776
-93.743713	-21.974599	1.856781
-93.555942	-18.548047	1.861786
-93.712948	-30.855435	1.866790
-93.819898	-30.646664	1.871795
-94.627128	-23.961636	1.876800
-95.321901	-17.006030	1.881805
-95.267240	-24.339161	1.886810
-94.958398	-23.175358	1.891814
-95.105428	-31.777112	1.896819
-95.193861	-31.552361	1.901824
-95.851367	-25.874490	1.906829
-96.475458	-30.311084	1.911834
-96.787822	-19.024263	1.916838
-97.042121	-17.884593	1.921843
-96.906768	-26.906134	1.926848
-97.372661	-36.266136	1.931853
-97.269988	-28.946287	1.936858
-97.853773	-24.589167	1.941862
-98.615824	-23.809138	1.946867
-98.254402	-41.397006	1.951872
-98.756505	-33.206513	1.956877
-98.613479	-26.744138	1.961882
-98.551123	-23.411006	1.966886
-98.979785	-24.421428	1.971891
-99.870427	-33.258601	1.976896
-100.267787	-30.656496	1.981901
-100.526337	-26.893662	1.986906
-100.526165	-28.861870	1.991910
-100.883861	-17.458443	1.996915
-100.766756	-34.415607	2.006912
-100.421997	-38.023697	2.016909
-99.654603	-34.285487	2.026906
-99.575747	-25.609469	2.036902
-99.343718	-28.640022	2.046899
-98.337084	-28.713732	2.056896
-97.496957	-35.515321	2.066893
-97.815764	-24.758727	2.076890
-97.243430	-24.401094	2.086886
-96.471343	-32.223020	2.096883
-96.229683	-26.525313	2.106880
-95.371818	-32.720153	2.116877
-94.581267	-29.219486	2.126874
-94.545685	-27.793723	2.136870
-94.342394	-26.237132	2.146867
-93.189287	-27.174695	2.156864
-92.970405	-22.410465	2.166861
-92.781402	-20.922437	2.176858
-91.794209	-35.876504	2.186854
-91.564194	-19.550405	2.196851
-91.403243	-23.465758	2.206848
-90.432402	-27.366785	2.216845
-89.972208	-28.258485	2.226842
-88.875114	-21.258749	2.236838
-88.967524	-22.014571	2.246835
-88.360674	-25.998380	2.256832
-88.352454	-32.301238	2.266829
-87.626751	-30.468849	2.276826
-87.060000	-30.224288	2.286822
-86.233991	-31.201140	2.296819
-85.437842	-30.367621	2.306816
-85.449823	-27.782002	2.316813
-85.441253	-30.462288	2.326810
-85.011862	-31.297629	2.336806
-84.311861	-31.705022	2.346803
-82.932714	-36.127724	2.356800
-82.755087	-29.204911	2.366797
-82.566518	-28.318986	2.376794
-81.973806	-25.219768	2.386790
-81.028791	-25.363107	2.396787
-80.849249	-28.683999	2.406784
-80.680576	-20.647220	2.416781
-80.084484	-27.771505	2.426778
-79.551629	-26.598421	2.436774
-79.297680	-29.580835	2.446771
-78.367646	-27.764630	2.456768
-77.951880	-26.454349	2.466765
-77.425624	-30.285554	2.476762
-76.330506	-26.874040	2.486758
-76.340649	-26.754618	2.496755
-76.269671	-25.289956	2.506752
-75.837540	-29.282920	2.516749
-74.921914	-34.355657	2.526746
-74.427357	-24.003255	2.536742
-73.535112	-27.498039	2.546739
-73.214804	-28.474787	2.556736
-73.121699	-27.631267	2.566733
-72.661744	-29.688850	2.576730
-72.012973	-26.505250	2.586726
-71.887847	-26.903180	2.596723
-70.502983	-31.848395	2.606720
-70.238077	-32.565474	2.616717
-69.924670	-37.770823	2.626714
-69.764353	-27.917251	2.636710
-68.737641	-31.950492	2.646707
-68.253874	-29.817728	2.656704
-68.185682	-24.445977	2.666701
-67.256760	-22.769165	2.676698
-67.081130	-31.003319	2.686694
-66.644388	-27.890276	2.696691
-65.653990	-23.193191	2.706688
-65.303535	-24.142816	2.716685
-65.145723	-19.112446	2.726682
-64.298408	-18.667097	2.736678
-64.128907	-26.233956	2.746675
-63.611872	-21.140266	2.756672
-62.824593	-23.956654	2.766669
-62.128239	-26.685707	2.776666
-62.012977	-28.419021	2.786662
-61.014540	-34.261717	2.796659
-60.580200	-23.653887	2.806656
-60.328793	-20.186800	2.816653
-60.286877	-33.777831	2.826650
-59.429418	-19.913738	2.836646
-58.952149	-23.229109	2.846643
-58.336649	-29.933121	2.856640
-57.474355	-31.045569	2.866637
-57.321936	-27.097948	2.876634
-57.343001	-17.460063	2.886630
-56.394721	-18.187839	2.896627
-55.803187	-31.373127	2.906624
-55.588230	-18.032091	2.916621
-54.671821	-28.916797	2.926618
-54.222047	-28.251254	2.936614
-54.383225	-31.864735	2.946611
-53.433276	-29.025968	2.956608
-52.720343	-20.714921	2.966605
-52.618491	-29.275213	2.976602
-51.569556	-28.804110	2.986598
-51.290378	-22.348519	2.996595
-51.228347	-33.189426	3.006592
-49.822395	-24.144965	3.016589
-49.364224	-33.625717	3.026586
-49.931415	-33.869721	3.036582
-49.321815	-21.361046	3.046579
-48.147661	-33.594440	3.056576
-47.949082	-26.412226	3.066573
-47.484544	-27.002270	3.076570
-46.624168	-19.694023	3.086566
-46.413221	-23.261431	3.096563
-46.089835	-30.102187	3.106560
-45.224982	-27.329664	3.116557
-44.873338	-23.309269	3.126554
-44.279118	-29.322241	3.136550
-43.365382	-28.078546	3.146547
-43.217790	-29.575680	3.156544
-42.849691	-33.867642	3.166541
-42.899340	-28.526301	3.176538
-41.764258	-35.485982	3.186534
-41.391362	-31.065083	3.196531
-40.672035	-31.727657	3.206528
-39.909009	-36.931544	3.216525
-39.646416	-31.517141	3.226522
-39.565761	-28.397405	3.236518
-39.244488	-32.335004	3.246515
-38.056794	-37.182728	3.256512
-37.760134	-28.425246	3.266509
-37.547499	-33.255463	3.276506
-36.652854	-25.394763	3.286502
-36.596817	-29.383557	3.296499
-35.951134	-36.328248	3.306496
-34.919707	-30.579689	3.316493
-35.109224	-26.109900	3.326490
-34.675448	-38.187646	3.336486
-33.408673	-35.003341	3.346483
-33.234579	-30.952419	3.356480
-33.181076	-42.283353	3.366477
-31.963426	-37.177721	3.376474
-31.732114	-31.316989	3.386470
-31.941328	-30.875139	3.396467
-30.673783	-33.620248	3.406464
-29.935446	-30.105115	3.416461
-30.043000	-28.415458	3.426458
-29.315931	-26.036331	3.436454
-28.908450	-26.688068	3.446451
-28.598341	-26.461445	3.456448
-27.620885	-25.459624	3.466445
-27.020888	-25.755554	3.476442
-27.193048	-12.131040	3.486438
-26.430916	-21.003156	3.496435
-25.856270	-18.350105	3.506432
-25.232858	-15.771988	3.516429
-24.307038	-26.608958	3.526426
-24.141309	-22.013054	3.536422
-24.056400	-23.091070	3.546419
-23.725660	-31.104497	3.556416
-22.656998	-21.906888	3.566413
-22.367555	-26.457603	3.576410
-21.593230	-12.551009	3.586406
-21.005276	-17.895380	3.596403
-20.785304	-27.099992	3.606400
-20.914088	-14.023084	3.616397
-19.682419	-25.869673	3.626394
-19.097374	-26.156119	3.636390
-19.034224	-30.370127	3.646387
-18.018675	-32.679450	3.656384
-17.669526	-22.235834	3.666381
-17.491694	-26.061319	3.676378
-16.741478	-19.368746	3.686374
-16.640340	-25.218838	3.696371
-15.628952	-27.911439	3.706368
-14.758590	-26.539958	3.716365
-14.497581	-26.014702	3.726362
-14.428021	-29.072835	3.736358
-14.454756	-24.910191	3.746355
-13.182460	-20.913320	3.756352
-12.826014	-27.900503	3.766349
-12.117602	-23.343999	3.776346
-11.250349	-21.068542	3.786342
-10.993911	-20.319086	3.796339
-10.969222	-21.854389	3.806336
-10.921644	-17.487789	3.816333
-9.510894	-22.231611	3.826330
-9.550234	-26.773729	3.836326
-8.472916	-19.370735	3.846323
-7.799093	-16.063835	3.856320
-7.759740	-24.477781	3.866317
-7.604943	-20.230053	3.876314
-7.035611	-19.014587	3.886310
-6.438569	-21.433841	3.896307
-5.695868	-9.991072	3.906304
-5.042968	-7.240312	3.916301
-5.129446	-5.552753	3.926298
-4.639914	-6.127465	3.936294
-4.235276	11.040197	3.946291
-3.649530	26.390483	3.956288
-3.212949	38.943220	3.966285
-2.709347	47.736786	3.976282
-2.181677	64.167708	3.986278
-1.600007	75.477521	3.996275
-1.519338	91.705453	4.006272
-0.812465	114.326180	4.016269
0.000000	132.555193	4.021274
0.202635	128.940763	4.026278
0.130979	146.115428	4.031283
0.161384	145.573611	4.036288
0.232736	140.120206	4.041293
0.061052	141.933179	4.046298
0.180207	147.351056	4.051302
0.235180	174.693515	4.056307
0.723497	165.265958	4.061312
0.894244	166.561816	4.066317
0.797415	161.874840	4.071322
0.521792	145.630954	4.076326
0.577153	147.491746	4.081331
0.612176	130.695856	4.086336
0.290785	142.306902	4.091341
0.789632	161.926437	4.096346
0.878399	151.790655	4.101350
0.512901	150.120613	4.106355
0.628948	145.566674	4.111360
0.440935	152.649931	4.116365
0.663623	165.889291	4.121370
1.174723	162.795497	4.126374
0.665902	154.867160	4.131379
0.359929	148.542713	4.136384
0.624726	159.897078	4.141389
0.613230	182.308220	4.146394
0.979542	170.708365	4.151398
0.675798	178.878622	4.156403
0.701481	175.597188	4.161408
0.851838	183.531398	4.166413
0.785545	180.771767	4.171418
1.048458	177.745522	4.176422
0.735085	175.611659	4.181427
0.556973	175.352816	4.186432
0.714304	178.145447	4.191437
0.671559	173.857477	4.196442
1.128772	171.344895	4.201446
1.016070	174.748933	4.206451
0.922988	164.704559	4.211456
0.666158	181.266127	4.216461
1.009629	168.847150	4.221466
1.085846	171.980725	4.226470
0.923806	183.754890	4.231475
1.047744	188.950013	4.236480
0.870196	182.729229	4.241485
1.073464	180.710362	4.246490
1.037186	177.476163	4.251494
0.726261	192.696364	4.256499
0.807644	176.832867	4.261504
0.938298	179.192560	4.266509
0.744695	184.850175	4.271514
0.855432	172.704557	4.276518
0.774194	185.248411	4.281523
0.656988	180.796049	4.286528
0.752237	182.860788	4.291533
1.092927	200.508802	4.296538
1.506853	193.367174	4.301542
1.440788	189.943442	4.306547
1.182389	177.601919	4.311552
0.972206	186.678866	4.316557
0.775539	187.404628	4.321562
1.297238	187.722218	4.326566
1.264740	198.866470	4.331571
1.553065	183.192622	4.336576
1.074246	190.126047	4.341581
0.937971	177.863196	4.346586
1.281804	183.727278	4.351590
1.305424	205.912646	4.356595
1.360050	195.162319	4.361600
1.409857	192.353507	4.366605
1.149221	192.656440	4.371610
1.295675	188.311944	4.376614
1.392822	198.352503	4.381619
1.641160	192.836880	4.386624
1.058747	189.489696	4.391629
0.972830	199.228329	4.396634
1.554545	193.511207	4.401638
1.557312	200.056453	4.406643
1.988708	196.447909	4.411648
1.516586	187.806415	4.416653
1.012694	195.387723	4.421658
1.291289	183.603560	4.426662
1.465858	194.748515	4.431667
1.358488	198.691332	4.436672
1.460503	205.187031	4.441677
1.314854	218.296897	4.446682
1.634503	211.014962	4.451686
1.315747	205.864257	4.456691
1.529535	200.353256	4.461696
1.753881	203.102754	4.466701
1.222084	203.174454	4.471706
1.754906	200.365339	4.476710
1.211758	215.720030	4.481715
1.235554	201.254132	4.486720
1.364873	198.934247	4.491725
1.441411	192.963890	4.496730
1.572733	210.589096	4.501734
1.432567	211.881089	4.506739
2.016788	212.582681	4.511744
1.958331	205.609382	4.516749
1.896069	208.231422	4.521754
1.975976	203.221525	4.526758
1.472949	211.087028	4.531763
1.805961	203.666149	4.536768
1.911607	204.978984	4.541773
1.905100	202.594724	4.546778
2.224529	208.734354	4.551782
1.923846	217.370379	4.556787
1.698282	204.747759	4.561792
1.586519	203.858384	4.566797
1.399278	199.876445	4.571802
1.698346	204.308820	4.576806
1.278378	211.440104	4.581811
1.536991	208.866809	4.586816
1.051694	215.083386	4.591821
1.514740	220.649470	4.596826
1.964556	230.304229	4.601830
1.818930	234.442897	4.606835
2.065706	226.187509	4.611840
2.181668	242.510054	4.616845
1.793490	231.792722	4.621850
2.013872	223.952112	4.626854
2.009207	231.226493	4.631859
2.059953	227.312656	4.636864
1.337231	215.372909	4.641869
1.603589	227.873858	4.646874
2.383085	227.931703	4.651878
2.438144	235.038563	4.656883
2.521004	225.235592	4.661888
2.502702	223.488435	4.666893
2.137240	206.438106	4.671898
2.536140	205.151501	4.676902
1.988517	200.792162	4.681907
2.142981	197.716551	4.686912
2.251262	194.718421	4.691917
2.186278	209.125906	4.696922
2.195536	200.409590	4.701926
1.886266	204.502484	4.706931
2.255321	198.646176	4.711936
2.022096	202.418002	4.716941
1.930120	208.250128	4.721946
2.167858	206.029529	4.726950
2.077837	219.433081	4.731955
2.243106	195.518095	4.736960
2.197341	206.657343	4.741965
2.269761	193.842140	4.746970
2.462636	199.272715	4.751974
2.057481	211.724994	4.756979
2.273950	203.110680	4.761984
2.113255	201.355683	4.766989
2.139321	200.366381	4.771994
2.438978	202.312696	4.776998
2.260419	214.220236	4.782003
1.955345	204.933532	4.787008
2.187739	220.384217	4.792013
2.629451	221.893586	4.797018
2.874319	224.830302	4.802022
2.398732	218.562466	4.807027
2.308401	211.051027	4.812032
2.359351	197.254573	4.817037
2.097833	205.276195	4.822042
2.538244	210.351644	4.827046
2.444691	234.852171	4.832051
2.708164	238.960627	4.837056
2.356247	217.026875	4.842061
2.518434	207.355932	4.847066
2.948645	208.101029	4.852070
2.467053	200.079771	4.857075
2.317882	208.312207	4.862080
2.242300	204.306585	4.867085
2.740035	223.385150	4.872090
2.757866	219.554003	4.877094
2.478327	226.153903	4.882099
2.448967	205.415077	4.887104
2.694097	210.825971	4.892109
2.486988	216.518682	4.897114
2.796941	219.144428	4.902118
2.576166	224.796583	4.907123
2.644618	232.675885	4.912128
2.680161	224.029304	4.917133
2.544715	225.509940	4.922138
2.879031	238.137887	4.927142
2.673540	242.337851	4.932147
2.789040	241.487772	4.937152
2.664706	236.983000	4.942157
2.880383	231.166134	4.947162
2.939065	225.122651	4.952166
2.259042	223.804297	4.957171
2.658592	228.555510	4.962176
2.612429	229.125583	4.967181
2.543976	234.106365	4.972186
3.053990	234.581766	4.977190
2.677516	230.385433	4.982195
2.780966	231.835273	4.987200
2.674056	235.718632	4.992205
2.317273	233.284616	4.997210
2.563655	230.415689	5.002214
2.746461	236.741975	5.007219
3.163801	233.688818	5.012224
2.673271	222.932665	5.017229
2.913161	228.304771	5.022234
3.002902	222.119220	5.027238
2.983810	231.463448	5.032243
3.200262	224.473223	5.037248
3.096685	230.008540	5.042253
3.105310	226.721232	5.047258
3.027223	218.849936	5.052262
2.994703	234.814811	5.057267
2.991166	230.804972	5.062272
2.747737	226.099287	5.067277
2.824665	226.560622	5.072282
3.285000	224.431885	5.077286
2.889623	232.917034	5.082291
3.057291	236.965158	5.087296
2.795200	235.640288	5.092301
3.007222	253.873157	5.097306
3.634812	255.576358	5.102310
3.200916	241.674313	5.107315
3.254542	220.950560	5.112320
2.943077	232.196085	5.117325
3.071300	231.537963	5.122330
3.311410	232.746891	5.127334
2.741282	239.822794	5.132339
3.272502	257.001250	5.137344
3.382644	255.652355	5.142349
3.176469	260.567902	5.147354
3.517643	246.849034	5.152358
3.181409	255.407097	5.157363
3.082357	257.279410	5.162368
2.887705	263.566958	5.167373
2.783959	263.614686	5.172378
3.073302	251.507762	5.177382
2.774140	256.240865	5.182387
2.736203	260.626048	5.187392
3.055794	271.309449	5.192397
3.380996	283.065918	5.197402
3.773270	287.355450	5.202406
3.511370	284.462181	5.207411
3.132956	270.755261	5.212416
3.132752	274.779835	5.217421
3.102186	289.380304	5.222426
3.363620	284.452162	5.227430
3.594679	293.949742	5.232435
3.697443	283.992894	5.237440
3.719316	285.207405	5.242445
3.757642	293.411170	5.247450
3.852555	281.304783	5.252454
3.119656	277.752771	5.257459
3.380457	271.229148	5.262464
3.859231	279.146428	5.267469
3.435261	288.821508	5.272474
3.829903	289.522763	5.277478
3.573350	283.954099	5.282483
3.689472	276.097937	5.287488
3.559174	265.627526	5.292493
3.429411	261.687275	5.297498
3.481802	277.304305	5.302502
3.492688	294.528636	5.307507
3.577205	295.621214	5.312512
3.955472	294.004449	5.317517
3.690200	300.050132	5.322522
3.977155	293.796347	5.327526
3.913528	287.314983	5.332531
3.763201	275.275370	5.337536
3.511348	271.521629	5.342541
3.430112	281.827316	5.347546
3.383291	282.755923	5.352550
3.702941	280.266057	5.357555
3.553921	289.544874	5.362560
3.668472	297.792774	5.367565
3.602969	294.473009	5.372570
3.916842	287.651344	5.377574
3.883812	294.814717	5.382579
3.959596	289.031010	5.387584
4.043573	285.834729	5.392589
3.825548	290.511420	5.397594
4.114868	289.930955	5.402598
3.779602	281.063951	5.407603
3.942535	287.500782	5.412608
3.577369	292.020061	5.417613
3.650588	302.890409	5.422618
4.293019	293.600289	5.427622
4.309379	293.913289	5.432627
3.870838	289.280178	5.437632
4.205830	286.205596	5.442637
4.152539	292.150243	5.447642
4.391321	304.310905	5.452646
4.036500	301.772471	5.457651
4.106370	292.501199	5.462656
4.353478	300.026429	5.467661
3.890518	292.813997	5.472666
3.752390	292.291245	5.477670
3.944682	290.310582	5.482675
3.796989	288.961771	5.487680
3.855236	286.131224	5.492685
3.724493	289.420471	5.497690
3.948441	291.819914	5.502694
3.554026	301.078418	5.507699
3.821101	293.988341	5.512704
4.141007	297.174508	5.517709
4.221381	305.502349	5.522714
4.488692	322.311607	5.527718
4.186931	310.553798	5.532723
4.143236	294.937761	5.537728
4.121751	299.289357	5.542733
4.108045	303.344780	5.547738
4.128183	308.465049	5.552742
3.953338	323.360506	5.557747
4.435196	320.542724	5.562752
4.523745	313.610986	5.567757
4.297078	314.464836	5.572762
4.590764	319.079074	5.577766
4.615247	317.616961	5.582771
4.235904	305.952580	5.587776
4.681099	295.490933	5.592781
4.360991	296.209278	5.597786
4.134971	284.912134	5.602790
4.223825	296.349148	5.607795
4.069735	316.182444	5.612800
4.692374	321.562366	5.617805
4.185006	313.651168	5.622810
4.426530	311.762110	5.627814
4.366290	326.001892	5.632819
4.403066	320.594981	5.637824
4.060687	308.460303	5.642829
4.585886	322.001721	5.647834
4.508911	309.252448	5.652838
4.660766	315.559314	5.657843
4.581158	317.651980	5.662848
4.663543	312.719479	5.667853
4.698317	315.772225	5.672858
4.486621	310.858035	5.677862
4.275189	321.181711	5.682867
4.770217	310.859017	5.687872
4.830116	334.889003	5.692877
4.584155	316.461960	5.697882
4.540922	313.868975	5.702886
4.812621	318.285682	5.707891
4.527560	318.566410	5.712896
4.721721	319.819442	5.717901
4.658168	323.757713	5.722906
5.011858	312.464297	5.727910
4.373460	331.049611	5.732915
4.990281	316.202556	5.737920
4.953488	312.788757	5.742925
4.496206	316.760620	5.747930
5.041207	330.301337	5.752934
4.981235	311.579951	5.757939
4.853976	313.737318	5.762944
4.782166	311.355941	5.767949
4.988178	310.292993	5.772954
4.913907	314.512137	5.777958
4.530809	317.153474	5.782963
4.350260	318.028807	5.787968
4.821533	316.249769	5.792973
4.356589	310.764861	5.797978
4.602096	319.438347	5.802982
4.765601	318.307049	5.807987
4.608960	326.364776	5.812992
4.720012	312.467916	5.817997
4.342658	322.045929	5.823002
4.852835	321.963001	5.828006
4.897226	337.254659	5.833011
4.929121	340.839159	5.838016
5.135988	347.418223	5.843021
4.870788	347.606285	5.848026
4.869511	352.300057	5.853030
4.983959	339.640968	5.858035
5.043808	351.938774	5.863040
5.313319	353.607533	5.868045
5.294891	359.072294	5.873050
5.330545	356.005137	5.878054
5.279321	352.432901	5.883059
5.267643	332.671150	5.888064
5.105465	315.923333	5.893069
4.869079	324.478647	5.898074
5.268630	337.535318	5.903078
5.046115	350.608078	5.908083
5.174364	342.891946	5.913088
5.228919	348.208889	5.918093
5.077172	344.701708	5.923098
5.190926	342.031572	5.928102
5.201676	354.354068	5.933107
5.408100	353.944363	5.938112
5.451784	344.455210	5.943117
5.134266	340.289652	5.948122
5.196081	332.692928	5.953126
4.991176	333.765460	5.958131
5.201393	352.502789	5.963136
5.241437	353.315921	5.968141
5.047692	349.927756	5.973146
5.031091	347.837071	5.978150
5.186772	351.538845	5.983155
4.992401	356.439251	5.988160
5.418987	350.237843	5.993165
5.263291	361.650401	5.998170
5.403259	350.539966	6.003174
5.153837	358.101302	6.008179
5.156359	361.506269	6.013184
5.559586	343.461259	6.018189
5.384228	353.704509	6.023194
5.798554	348.844411	6.028198
5.350252	352.291417	6.033203
5.418326	356.596264	6.038208
5.393419	343.790706	6.043213
5.120009	352.269084	6.048218
5.129036	336.563394	6.053222
5.143532	352.786505	6.058227
5.626621	366.618957	6.063232
5.691136	372.484874	6.068237
5.154553	367.342783	6.073242
5.577075	361.553545	6.078246
5.183695	352.643419	6.083251
5.495590	367.014126	6.088256
5.942485	369.301660	6.093261
5.590719	350.320041	6.098266
5.505437	345.368176	6.103270
5.332222	352.366009	6.108275
5.375342	334.155085	6.113280
5.429503	345.814522	6.118285
5.153799	338.299617	6.123290
5.506540	345.042714	6.128294
5.639324	345.775801	6.133299
5.500418	347.067892	6.138304
5.723665	343.830333	6.143309
5.522070	351.377646	6.148314
5.530566	345.412160	6.153318
5.485985	358.905207	6.158323
5.020204	355.962744	6.163328
5.386482	354.641264	6.168333
5.050142	343.886084	6.173338
5.190265	345.308762	6.178342
5.133429	349.602580	6.183347
5.070101	371.073865	6.188352
5.614948	377.510369	6.193357
5.396944	383.108355	6.198362
5.544136	370.309655	6.203366
5.684823	375.664958	6.208371
5.961900	378.958260	6.213376
5.707618	352.069247	6.218381
5.444717	358.030602	6.223386
5.381083	347.728677	6.228390
5.809021	345.543123	6.233395
5.558520	340.376752	6.238400
5.889062	343.091757	6.243405
5.545371	355.602858	6.248410
5.355069	354.655714	6.253414
5.557382	351.537832	6.258419
5.417254	362.661907	6.263424
5.371725	349.185423	6.268429
5.631733	348.018838	6.273434
5.699317	345.724030	6.278438
5.733447	352.305792	6.283443
5.730612	352.656792	6.288448
5.546580	340.934160	6.293453
5.358219	326.196476	6.298458
5.070331	317.353192	6.303462
5.102010	321.904276	6.308467
5.699955	334.383666	6.313472
5.515225	346.059988	6.318477
5.439684	353.480414	6.323482
5.500861	344.615342	6.328486
5.389901	344.101516	6.333491
5.740489	345.169367	6.338496
5.340841	333.626018	6.343501
5.273336	322.167392	6.348506
5.267439	323.967295	6.353510
5.482351	342.294603	6.358515
5.537197	342.064643	6.363520
5.595317	337.831584	6.368525
5.153315	340.032581	6.373530
5.509607	353.842467	6.378534
5.478779	342.029305	6.383539
5.438438	335.053644	6.388544
5.456975	328.237751	6.393549
5.727996	332.407041	6.398554
5.192057	318.309772	6.403558
5.027855	328.567046	6.408563
5.338342	334.220044	6.413568
5.539209	339.037668	6.418573
5.171116	354.052007	6.423578
5.035987	353.132446	6.428582
5.195498	339.541090	6.433587
5.516639	348.521845	6.438592
5.693501	341.835267	6.443597
5.072953	344.223721	6.448602
5.573895	335.155359	6.453606
5.427177	345.732268	6.458611
5.528910	343.720491	6.463616
5.809569	339.990316	6.468621
5.493005	337.252874	6.473626
5.226604	345.963220	6.478630
5.488733	346.369782	6.483635
5.519147	343.261564	6.488640
5.392434	348.421701	6.493645
5.086489	350.022770	6.498650
5.006623	336.228077	6.503654
5.213525	342.753759	6.508659
5.589856	351.733979	6.513664
5.683063	346.683459	6.518669
5.282866	353.208049	6.523674
5.255463	354.398053	6.528678
5.382573	344.258275	6.533683
5.105729	356.663618	6.538688
5.275027	343.243588	6.543693
5.314154	348.000039	6.548698
5.374307	354.410473	6.553702
5.132332	350.688328	6.558707
5.458615	346.451797	6.563712
5.504094	348.923263	6.568717
5.385452	353.665436	6.573722
5.585817	358.604794	6.578726
5.570269	344.386877	6.583731
5.406256	353.399861	6.588736
5.747028	343.167356	6.593741
5.608148	356.549997	6.598746
5.630385	348.916199	6.603750
5.589469	346.961834	6.608755
5.841537	349.525936	6.613760
6.196626	335.796699	6.618765
5.300039	351.397875	6.623770
5.703111	344.757773	6.628774
5.869164	340.085213	6.633779
5.495876	336.797754	6.638784
5.580926	319.848660	6.643789
5.275846	321.095696	6.648794
5.418141	311.248220	6.653798
5.390460	318.604485	6.658803
5.202674	309.059386	6.663808
5.327185	305.729331	6.668813
4.860381	324.127343	6.673818
5.538687	325.597625	6.678822
5.464842	340.343022	6.683827
5.717442	344.655158	6.688832
5.746148	339.985563	6.693837
5.561452	329.907088	6.698842
5.334388	309.976540	6.703846
5.350066	311.002259	6.708851
5.374407	321.883558	6.713856
5.841326	311.384274	6.718861
5.290137	319.116808	6.723866
5.543266	317.838300	6.728870
5.581306	312.113800	6.733875
5.265722	321.615406	6.738880
5.378474	311.526956	6.743885
5.146058	328.748715	6.748890
5.565115	312.570299	6.753894
5.413582	316.078851	6.758899
5.325298	319.508187	6.763904
5.293331	310.377747	6.768909
5.255747	326.037122	6.773914
5.564511	329.830799	6.778918
5.736259	335.680955	6.783923
5.500029	335.062041	6.788928
5.395261	317.824763	6.793933
5.110137	325.540956	6.798938
5.211085	323.442689	6.803942
5.538289	343.661756	6.808947
5.681334	347.360487	6.813952
5.406874	333.491304	6.818957
5.021687	333.232739	6.823962
5.718024	327.174706	6.828966
5.914898	335.169283	6.833971
5.941786	329.105856	6.838976
5.853590	314.845709	6.843981
5.765001	314.267710	6.848986
5.724735	316.435662	6.853990
5.927217	321.998966	6.858995
5.785869	315.501725	6.864000
5.592159	305.994110	6.869005
5.348513	286.610824	6.874010
5.309456	281.840469	6.879014
5.152864	285.355572	6.884019
5.640938	290.358058	6.889024
5.358574	294.211132	6.894029
5.071333	302.580680	6.899034
5.336617	307.142780	6.904038
5.575350	309.165869	6.909043
5.460912	315.836097	6.914048
5.765157	307.966294	6.919053
5.515617	317.301498	6.924058
5.543459	310.111839	6.929062
5.494466	295.818495	6.934067
5.268960	293.635269	6.939072
5.613106	286.908542	6.944077
5.310005	291.541182	6.949082
5.539912	295.126099	6.954086
5.210456	293.092450	6.959091
5.325905	288.492297	6.964096
5.530143	281.817401	6.969101
5.603928	294.384364	6.974106
5.494946	293.746101	6.979110
5.432533	299.467220	6.984115
5.550644	303.282333	6.989120
5.441941	292.325800	6.994125
5.224664	288.844852	6.999130
5.602240	291.469991	7.004134
5.389222	290.791403	7.009139
5.384900	293.396385	7.014144
5.510330	283.568289	7.019149
5.339178	282.971279	7.024154
5.378634	284.994443	7.029158
5.377005	284.476067	7.034163
5.431091	300.397496	7.039168
5.570235	282.876265	7.044173
5.484050	288.869855	7.049178
5.533130	278.545009	7.054182
5.416157	299.270230	7.059187
5.353618	299.756686	7.064192
5.564807	295.637550	7.069197
5.410625	297.414204	7.074202
5.081188	286.415620	7.079206
5.298248	287.124319	7.084211
5.252848	297.390058	7.089216
5.797002	307.428840	7.094221
5.199441	298.608229	7.099226
5.299462	305.573812	7.104230
5.821505	297.090677	7.109235
5.146778	309.757174	7.114240
5.722687	293.065982	7.119245
5.519304	286.725314	7.124250
5.123681	290.789289	7.129254
5.130720	300.756507	7.134259
5.205117	320.054912	7.139264
5.308381	312.851111	7.144269
5.165231	317.064669	7.149274
5.363317	314.286580	7.154278
5.614406	325.674312	7.159283
5.323912	317.908508	7.164288
5.190073	318.546052	7.169293
5.239895	315.075912	7.174298
5.454402	324.122518	7.179302
5.300054	321.364883	7.184307
5.608851	316.172294	7.189312
5.577986	311.116836	7.194317
5.486533	322.219815	7.199322
5.761204	326.922733	7.204326
5.248171	322.485130	7.209331
5.565351	322.782950	7.214336
6.009679	317.787675	7.219341
5.562206	327.000603	7.224346
5.570339	312.010750	7.229350
5.389469	311.775840	7.234355
4.933725	304.160081	7.239360
5.693798	312.281090	7.244365
5.309472	326.037926	7.249370
5.801418	321.026001	7.254374
5.459367	312.541019	7.259379
5.146447	320.241874	7.264384
5.550353	308.825028	7.269389
5.535086	322.906133	7.274394
5.567279	307.846404	7.279398
5.526492	301.867770	7.284403
5.176836	307.139025	7.289408
5.496559	290.818208	7.294413
5.459211	293.990405	7.299418
5.177869	291.508594	7.304422
5.087624	304.610069	7.309427
5.215599	319.011519	7.314432
5.713626	310.211805	7.319437
5.529265	321.329644	7.324442
5.791715	315.503635	7.329446
5.537763	304.714446	7.334451
5.266890	305.519662	7.339456
5.508732	295.490790	7.344461
5.271109	290.919582	7.349466
5.301058	307.347273	7.354470
5.729093	311.077925	7.359475
5.322043	310.751940	7.364480
5.477979	305.450145	7.369485
5.411532	310.261914	7.374490
5.991424	301.900235	7.379494
5.536509	288.239090	7.384499
5.212573	296.990189	7.389504
5.392268	296.224901	7.394509
5.176293	286.622616	7.399514
5.414104	286.211377	7.404518
5.337941	283.722101	7.409523
5.221832	288.136982	7.414528
5.312879	291.146190	7.419533
5.617669	317.238471	7.424538
5.253691	308.464396	7.429542
5.268469	314.045891	7.434547
5.201392	319.175051	7.439552
5.720931	312.568302	7.444557
5.413938	304.267545	7.449562
5.384843	314.723181	7.454566
5.286476	316.194639	7.459571
5.164955	332.957569	7.464576
5.504310	316.892852	7.469581
5.167790	318.540998	7.474586
5.211320	308.644830	7.479590
5.511782	312.252030	7.484595
4.917709	327.191610	7.489600
5.409147	313.052233	7.494605
5.424227	310.836450	7.499610
5.599464	321.932453	7.504614
5.336628	318.539236	7.509619
5.377345	321.842677	7.514624
5.342201	320.079744	7.519629
5.221881	323.853759	7.524634
5.373157	326.250418	7.529638
5.239081	320.225038	7.534643
4.982141	318.752308	7.539648
5.312058	324.327704	7.544653
5.530340	336.908806	7.549658
6.007094	352.680726	7.554662
5.823099	330.689366	7.559667
5.187059	318.889612	7.564672
5.304029	319.006331	7.569677
5.104573	317.567906	7.574682
5.017881	323.372762	7.579686
5.557964	335.429692	7.584691
5.096773	345.002828	7.589696
5.498662	337.918964	7.594701
5.576152	342.638785	7.599706
5.370787	353.664025	7.604710
5.586148	353.116498	7.609715
5.399761	369.220297	7.614720
5.597212	351.446161	7.619725
5.474397	351.338792	7.624730
5.193756	339.496374	7.629734
5.170576	343.224644	7.634739
5.382145	356.401978	7.639744
5.403803	349.645050	7.644749
5.526610	362.620897	7.649754
5.646310	349.346588	7.654758
5.599401	356.153661	7.659763
5.499215	358.465203	7.664768
5.696722	334.859786	7.669773
5.081953	324.983601	7.674778
5.039891	321.893283	7.679782
5.317756	337.076607	7.684787
5.447067	352.326721	7.689792
5.851656	347.217543	7.694797
5.843674	347.707515	7.699802
5.477633	334.397565	7.704806
5.490075	321.496075	7.709811
5.450196	323.397192	7.714816
5.874260	315.909122	7.719821
5.508952	322.873078	7.724826
5.195517	315.077227	7.729830
5.160471	324.336737	7.734835
5.090785	332.142135	7.739840
5.376974	313.966342	7.744845
5.344242	327.699411	7.749850
5.656899	326.551653	7.754854
5.604500	321.888560	7.759859
5.090752	318.216859	7.764864
5.688557	318.778091	7.769869
5.408690	327.464605	7.774874
5.712369	314.069652	7.779878
5.681302	319.853376	7.784883
5.532348	328.710246	7.789888
5.674700	314.627174	7.794893
5.610106	315.674052	7.799898
5.685986	320.917512	7.804902
5.862974	317.232198	7.809907
5.790271	318.117828	7.814912
5.622405	313.499865	7.819917
5.700220	317.726335	7.824922
5.414324	310.332899	7.829926
5.692242	298.625812	7.834931
5.124173	296.826936	7.839936
5.348108	283.607775	7.844941
5.455453	290.009594	7.849946
5.425468	293.835070	7.854950
5.345529	297.387627	7.859955
5.336970	308.007089	7.864960
5.551812	311.438916	7.869965
5.603873	315.428127	7.874970
5.257138	294.251693	7.879974
5.270264	295.953737	7.884979
5.681835	311.224747	7.889984
5.535849	302.818755	7.894989
5.585966	306.561837	7.899994
5.330283	299.352738	7.904998
5.325437	293.175588	7.910003
5.432017	297.864838	7.915008
5.462621	281.701812	7.920013
5.323253	300.291441	7.925018
5.102036	295.121332	7.930022
5.529164	307.566774	7.935027
5.461170	315.998559	7.940032
5.639777	317.200293	7.945037
5.338049	301.561086	7.950042
5.183820	311.389018	7.955046
5.362879	313.821337	7.960051
5.597431	330.157921	7.965056
5.765282	322.761516	7.970061
5.514690	319.646760	7.975066
5.039627	301.087509	7.980070
5.453645	303.074133	7.985075
5.352950	330.734326	7.990080
5.566961	325.848538	7.995085
5.435240	331.895940	8.000090
5.664943	325.257958	8.005094
5.453547	311.270245	8.010099
5.191334	314.275483	8.015104
5.560623	302.006532	8.020109
5.258690	304.022061	8.025126
5.513622	307.323775	8.030144
5.252296	302.994479	8.035162
5.502456	330.717476	8.040179
5.578562	323.542199	8.045197
5.545019	319.502359	8.050214
5.352981	306.335262	8.055232
5.533652	304.999261	8.060250
5.579802	318.697651	8.065267
5.328583	309.561310	8.070285
5.506834	306.160753	8.075302
5.676989	311.524998	8.080320
5.599253	298.041046	8.085338
5.180236	284.003188	8.090355
5.320858	301.323629	8.095373
5.718378	314.614609	8.100390
5.603439	315.474878	8.105408
5.336184	302.938795	8.110426
5.394849	319.641525	8.115443
5.908189	318.217680	8.120461
5.558635	317.997546	8.125478
5.434268	294.939981	8.130496
5.725861	313.051076	8.135514
5.633571	299.331975	8.140531
5.650536	306.631990	8.145549
5.394107	301.887497	8.150566
5.237615	304.901854	8.155584
5.601005	304.959300	8.160602
5.519113	314.963424	8.165619
5.707595	306.567257	8.170637
5.881094	330.742096	8.175654
5.308992	304.472522	8.180672
5.772576	305.849963	8.185690
5.441744	297.001142	8.190707
5.503922	307.108593	8.195725
5.820738	314.063547	8.200742
5.585517	319.845406	8.205760
5.640223	301.796148	8.210778
5.278676	315.290405	8.215795
5.594315	315.114352	8.220813
5.747302	322.933033	8.225830
5.793789	326.889550	8.230848
5.775473	320.472256	8.235866
5.675895	326.709464	8.240883
5.745674	315.748760	8.245901
5.663833	313.259027	8.250918
5.320337	319.459390	8.255936
5.891180	316.228358	8.260954
5.603890	327.999465	8.265971
5.810456	311.305150	8.270989
5.879655	318.095750	8.276006
5.202379	321.928905	8.281024
5.426005	319.498907	8.286042
5.432916	330.253080	8.291059
5.629089	328.349958	8.296077
5.905896	321.747010	8.301094
5.774851	330.137629	8.306112
5.935588	326.532423	8.311130
5.710660	336.137444	8.316147
5.821424	326.432021	8.321165
5.638977	316.878975	8.326182
5.712948	328.536751	8.331200
5.977337	313.372052	8.336218
5.780720	324.651394	8.341235
5.945726	326.675898	8.346253
5.587833	332.405016	8.351270
5.500542	333.078862	8.356288
5.893238	321.206196	8.361306
5.768779	324.711133	8.366323
5.991991	329.594267	8.371341
5.715496	321.189318	8.376358
5.341736	322.943670	8.381376
5.605846	318.388197	8.386394
5.477743	324.549622	8.391411
5.416379	326.052783	8.396429
5.632967	326.644430	8.401446
5.599443	325.441836	8.406464
5.897788	329.184227	8.411482
5.545710	331.196267	8.416499
5.776658	339.321008	8.421517
6.164156	347.741672	8.426534
5.654468	338.965288	8.431552
5.976931	324.311551	8.436570
5.733319	326.888329	8.441587
5.596558	324.520247	8.446605
5.999580	353.351960	8.451622
5.844489	356.471095	8.456640
6.173348	359.187090	8.461658
5.647060	349.774686	8.466675
6.125275	348.087797	8.471693
5.905670	341.670004	8.476710
5.793549	333.484787	8.481728
6.199073	337.833759	8.486746
5.800582	338.855432	8.491763
6.104248	326.895524	8.496781
5.700637	320.712439	8.501798
5.333422	338.337568	8.506816
6.130687	341.279640	8.511834
6.215505	355.924444	8.516851
6.105663	360.203795	8.521869
5.838159	356.957976	8.526886
5.747515	357.299763	8.531904
5.924729	355.788771	8.536922
5.604716	362.383325	8.541939
5.981008	361.039988	8.546957
6.042862	359.221743	8.551974
5.785708	359.713366	8.556992
5.955502	357.349235	8.562010
6.078483	362.878351	8.567027
5.756702	365.783348	8.572045
6.005624	358.452356	8.577063
5.757348	358.545540	8.582080
5.922867	357.246382	8.587098
5.637998	363.756305	8.592115
5.655278	352.751012	8.597133
6.084676	348.941789	8.602151
5.892317	375.100608	8.607168
5.940828	364.847680	8.612186
5.928091	376.081912	8.617203
6.104308	379.902951	8.622221
6.272488	393.354021	8.627239
6.179276	390.583629	8.632256
5.921037	369.796668	8.637274
5.916499	377.841370	8.642291
6.247377	385.139637	8.647309
6.205325	384.760045	8.652327
5.724530	378.685736	8.657344
6.203827	387.776261	8.662362
6.264829	396.163423	8.667379
6.181002	392.860968	8.672397
6.293525	389.722979	8.677415
6.170424	382.893528	8.682432
5.758275	374.683867	8.687450
6.001130	379.092502	8.692467
5.704258	380.867712	8.697485
6.289000	390.007237	8.702503
6.358146	395.287928	8.707520
6.557819	393.495813	8.712538
6.472888	398.233273	8.717555
6.058271	379.118486	8.722573
6.318873	371.600947	8.727591
6.308329	377.921968	8.732608
6.247056	371.645880	8.737626
5.953932	365.513304	8.742643
5.716694	367.665100	8.747661
6.120557	378.351053	8.752679
6.092328	380.586400	8.757696
6.323637	400.579747	8.762714
6.285189	389.965258	8.767731
5.959869	401.096272	8.772749
6.425943	383.105982	8.777767
6.341072	391.254304	8.782784
6.504848	385.592177	8.787802
6.247213	393.497743	8.792819
5.970930	404.826128	8.797837
6.387587	396.128477	8.802855
6.084997	399.561410	8.807872
6.114717	390.719672	8.812890
6.481238	388.902347	8.817907
6.340136	382.285772	8.822925
6.332078	392.480561	8.827943
6.177007	396.522559	8.832960
6.321871	392.136545	8.837978
6.298206	396.688520	8.842995
5.800355	390.351819	8.848013
6.200023	392.750074	8.853031
6.461544	396.892686	8.858048
6.426939	387.141280	8.863066
6.035131	400.321184	8.868083
5.896780	399.406329	8.873101
6.138693	390.917150	8.878119
6.075847	403.262133	8.883136
6.330631	413.792071	8.888154
6.361625	416.072055	8.893171
6.076697	422.034477	8.898189
6.700904	421.043991	8.903207
6.422719	433.661842	8.908224
6.316504	427.351433	8.913242
6.506503	415.702903	8.918259
6.263185	428.340082	8.923277
6.705475	429.195660	8.928295
6.338141	431.079942	8.933312
6.438533	433.586408	8.938330
6.383901	432.849217	8.943347
6.179125	426.564542	8.948365
6.624588	419.109623	8.953383
6.257405	426.496794	8.958400
6.554295	439.767511	8.963418
6.534226	425.818883	8.968435
6.307258	436.604301	8.973453
6.469298	425.612527	8.978471
6.499310	431.928344	8.983488
6.681520	426.987333	8.988506
6.536398	434.101930	8.993523
6.345219	425.362511	8.998541
6.633943	429.039993	9.003559
6.377027	424.076587	9.008576
6.478922	427.490805	9.013594
6.378958	432.083740	9.018611
6.319462	426.618012	9.023629
6.532223	422.822626	9.028647
6.101496	425.569981	9.033664
6.243096	425.810509	9.038682
6.426601	433.870614	9.043699
5.921574	423.760291	9.048717
6.702845	423.879072	9.053735
6.230294	428.234911	9.058752
6.355990	438.882441	9.063770
6.507059	446.424683	9.068787
6.696995	446.651024	9.073805
6.505711	440.935367	9.078823
6.396592	446.665634	9.083840
6.653794	454.489301	9.088858
6.719345	448.980464	9.093875
6.611377	452.648521	9.098893
6.885676	445.072492	9.103911
6.801982	446.982135	9.108928
6.818595	451.631880	9.113946
6.729502	450.259260	9.118963
6.539825	443.381542	9.123981
6.840997	438.386623	9.128999
6.744160	441.425788	9.134016
6.689440	452.281061	9.139034
6.698449	434.388285	9.144051
6.443348	439.091096	9.149069
6.758397	434.080698	9.154087
6.829856	444.134255	9.159104
6.707481	449.255309	9.164122
6.671538	437.709738	9.169139
6.866083	451.010662	9.174157
6.663995	434.922229	9.179175
6.950302	433.028997	9.184192
6.713619	438.795889	9.189210
6.587632	426.787243	9.194227
6.670744	435.102379	9.199245
6.787963	444.268812	9.204263
6.930320	450.366897	9.209280
6.646500	454.011857	9.214298
6.820772	437.222762	9.219315
6.761463	458.215018	9.224333
7.010230	446.028209	9.229351
6.650574	445.191941	9.234368
6.793053	448.558815	9.239386
6.628720	443.712854	9.244403
6.791642	452.079464	9.249421
7.018696	455.598967	9.254439
6.812754	457.448217	9.259456
6.687101	460.214639	9.264474
6.791101	451.525620	9.269491
6.941682	457.259718	9.274509
6.901182	446.570346	9.279527
7.027333	455.257248	9.284544
6.925664	451.290136	9.289562
7.311011	450.239532	9.294579
7.043546	440.565837	9.299597
6.910548	427.718346	9.304615
7.082181	428.934930	9.309632
7.160050	434.369675	9.314650
6.842543	436.845712	9.319667
6.930668	424.512466	9.324685
6.638677	417.935080	9.329703
6.657876	425.350903	9.334720
6.609795	424.557029	9.339738
7.063714	425.938735	9.344755
6.970802	434.174121	9.349773
6.676462	430.837070	9.354791
6.440981	426.187483	9.359808
6.622304	445.830259	9.364826
7.086401	441.660719	9.369843
6.847740	450.105991	9.374861
7.032565	453.620171	9.379879
7.027951	462.734911	9.384896
6.847331	452.959078	9.389914
7.293650	439.114434	9.394931
7.165296	449.475668	9.399949
7.213583	451.660101	9.404967
7.326130	447.530447	9.409984
7.000663	454.425296	9.415002
7.263251	437.534712	9.420019
7.170678	448.120698	9.425037
7.290627	445.828755	9.430055
7.193262	435.023320	9.435072
6.616578	435.746258	9.440090
7.118230	425.611677	9.445107
7.175460	441.943684	9.450125
7.267118	436.036713	9.455143
7.287613	433.850462	9.460160
7.450687	427.024478	9.465178
7.120279	427.397524	9.470195
6.977188	427.932296	9.475213
6.922286	425.374030	9.480231
7.151693	419.599784	9.485248
6.600607	431.838893	9.490266
7.269019	443.462981	9.495283
7.179785	449.625413	9.500301
7.134387	443.492019	9.505319
7.201641	438.586829	9.510336
7.170752	436.574196	9.515354
7.265849	439.783574	9.520371
7.193204	425.269528	9.525389
7.094293	432.723077	9.530407
7.325442	432.586670	9.535424
6.958468	432.014851	9.540442
7.176417	437.869182	9.545459
7.513325	450.041962	9.550477
6.718236	447.087699	9.555495
7.023666	435.958267	9.560512
6.737674	446.714870	9.565530
6.977661	450.696913	9.570547
7.029724	457.028975	9.575565
7.091095	446.392146	9.580583
7.237579	453.559628	9.585600
7.140446	455.137007	9.590618
7.387414	454.909123	9.595635
7.247627	450.756121	9.600653
6.827192	446.821119	9.605671
7.046567	441.918933	9.610688
7.065554	456.343947	9.615706
7.553687	480.702516	9.620723
7.419838	483.470297	9.625741
7.424007	486.599157	9.630759
7.561627	465.492956	9.635776
7.397622	456.328436	9.640794
7.360326	443.012740	9.645811
7.064269	449.598944	9.650829
7.324933	447.401934	9.655847
7.104952	453.330116	9.660864
7.066518	470.072869	9.665882
7.565935	483.702014	9.670899
7.192460	484.701947	9.675917
7.247926	481.420738	9.680935
7.410982	484.490671	9.685952
7.120619	492.318639	9.690970
7.469545	494.878123	9.695987
7.676986	499.463971	9.701005
7.336216	484.018174	9.706023
7.711741	484.480038	9.711040
7.335239	494.521843	9.716058
7.575748	484.343584	9.721075
7.610110	489.478704	9.726093
7.766436	489.058061	9.731111
7.960790	473.678145	9.736128
7.366424	471.581786	9.741146
7.907156	454.767539	9.746163
7.428107	448.906358	9.751181
7.168106	446.387493	9.756199
7.508274	442.159805	9.761216
7.465154	452.312995	9.766234
7.597134	450.575654	9.771251
7.602430	443.720037	9.776269
7.207410	442.344439	9.781287
7.864218	444.811705	9.786304
7.329577	452.822810	9.791322
7.699098	449.647358	9.796339
7.637123	454.622238	9.801357
7.450548	462.145495	9.806375
7.948553	452.765299	9.811392
7.907283	455.339462	9.816410
7.495602	442.914025	9.821427
7.661641	446.558351	9.826445
7.497618	460.343066	9.831463
7.310376	453.595626	9.836480
7.323336	455.184334	9.841498
7.559264	445.579587	9.846515
7.481835	441.815027	9.851533
7.571592	482.404173	9.856551
7.995635	473.343808	9.861568
7.731815	480.430610	9.866586
7.695280	462.141366	9.871603
7.443875	459.331072	9.876621
7.492573	470.442348	9.881639
7.893250	476.092513	9.886656
7.675438	476.504718	9.891674
7.651357	479.139714	9.896691
7.709818	480.235266	9.901709
7.525962	482.364873	9.906727
7.786671	476.281256	9.911744
7.653456	487.639889	9.916762
7.906844	481.187174	9.921779
7.772720	479.595360	9.926797
7.685273	479.549094	9.931815
8.072219	474.805098	9.936832
7.741002	474.810924	9.941850
7.876238	468.458137	9.946867
7.981096	471.205364	9.951885
7.622096	467.143395	9.956903
7.575855	468.017512	9.961920
7.984911	476.253615	9.966938
7.826114	473.842113	9.971955
8.251049	487.945198	9.976973
7.737462	468.195198	9.981991
7.660503	462.126844	9.987008
7.954167	460.868399	9.992026
7.798449	454.111617	9.997043
7.535111	453.463726	10.002061
7.459114	470.451718	10.007079
8.106415	470.450734	10.012096
7.858808	483.216597	10.017114
7.872484	492.316523	10.022131
7.981805	478.748557	10.027149
7.672258	473.936818	10.032167
7.884719	473.782832	10.037184
7.984907	480.738529	10.042202
8.061898	495.463485	10.047219
7.921024	485.316759	10.052237
7.565690	482.069387	10.057255
7.659102	478.599068	10.062272
7.832625	479.181207	10.067290
7.637117	473.496447	10.072307
7.755483	478.379438	10.077325
7.593847	485.046279	10.082343
7.987242	480.397950	10.087360
8.106109	474.653071	10.092378
7.557568	476.665219	10.097395
7.864002	478.024658	10.102413
7.921287	497.457331	10.107431
8.022864	509.312910	10.112448
8.023690	518.781445	10.117466
8.153258	510.512501	10.122483
8.315327	495.022270	10.127501
7.896552	497.799940	10.132519
8.044304	492.223380	10.137536
7.953576	495.237633	10.142554
8.079292	500.126895	10.147571
8.634343	502.052130	10.152589
8.133637	498.440068	10.157607
8.126849	487.290258	10.162624
8.129974	484.043285	10.167642
8.014452	478.460835	10.172659
8.378508	467.968720	10.177677
8.115082	470.636378	10.182695
8.173781	475.509153	10.187712
8.014144	480.738917	10.192730
7.960622	491.052582	10.197747
8.123888	474.703472	10.202765
8.005592	473.007881	10.207783
7.990371	479.727971	10.212800
8.090855	497.379616	10.217818
8.111153	508.224500	10.222835
8.628028	502.092735	10.227853
8.460883	505.326176	10.232871
8.197464	486.970280	10.237888
8.245302	475.827295	10.242906
7.989563	478.946850	10.247923
8.221806	472.379446	10.252941
8.353074	483.500900	10.257959
8.379382	487.468469	10.262976
8.076205	484.465877	10.267994
8.050179	483.999397	10.273011
8.486227	490.179255	10.278029
8.295566	504.847288	10.283047
8.435510	497.412115	10.288064
8.638133	493.699475	10.293082
8.362666	486.277453	10.298099
8.316981	478.667884	10.303117
7.944794	477.395183	10.308135
8.284933	478.624666	10.313152
8.336886	484.487847	10.318170
8.116097	491.638199	10.323187
8.882783	503.681644	10.328205
8.432599	494.514205	10.333223
8.154518	478.635491	10.338240
8.226346	480.809346	10.343258
8.269728	492.654257	10.348275
8.426389	495.227602	10.353293
8.213632	504.852563	10.358311
8.213616	506.682058	10.363328
8.316481	511.173992	10.368346
8.396636	510.600217	10.373363
8.775066	503.478816	10.378381
8.620796	508.215959	10.383399
8.499292	503.102614	10.388416
8.576769	511.679306	10.393434
8.821389	515.329753	10.398451
8.903752	492.307993	10.403469
8.585928	480.933750	10.408487
8.515471	477.110265	10.413504
8.249080	475.037842	10.418522
8.252475	479.340139	10.423539
8.401669	467.121450	10.428557
8.230838	482.307348	10.433575
8.478000	484.333747	10.438592
8.691350	498.433231	10.443610
8.471794	508.491326	10.448627
8.774555	498.227784	10.453645
8.482823	508.125986	10.458663
8.650190	506.894018	10.463680
8.641614	514.053596	10.468698
8.907521	506.145125	10.473715
8.726235	485.277390	10.478733
9.080344	475.213017	10.483751
8.741335	472.059192	10.488768
8.635580	480.648727	10.493786
8.586569	473.940137	10.498803
8.625481	476.958156	10.503821
9.027128	489.737774	10.508839
8.856005	474.801353	10.513856
8.941258	479.555884	10.518874
8.451089	477.168339	10.523891
8.591265	469.063185	10.528909
8.762220	481.814888	10.533927
8.901846	475.179928	10.538944
8.768740	470.772418	10.543962
8.709098	478.896444	10.548979
8.806558	475.024250	10.553997
8.593695	478.124222	10.559015
8.462965	480.940789	10.564032
8.717046	488.085094	10.569050
8.218767	483.341442	10.574067
8.567003	473.896235	10.579085
8.692210	478.602833	10.584103
8.588631	467.977993	10.589120
8.601877	476.774691	10.594138
8.797510	487.155133	10.599155
8.745323	476.663502	10.604173
8.789134	492.633969	10.609191
8.777535	499.914883	10.614208
8.762991	501.471533	10.619226
8.827109	502.274374	10.624243
9.081763	503.775714	10.629261
8.926504	504.915835	10.634279
8.835809	497.692465	10.639296
8.836850	504.924156	10.644314
8.666781	503.355698	10.649331
9.031103	499.465083	10.654349
8.959561	505.562814	10.659367
8.611554	507.447454	10.664384
9.167081	507.380058	10.669402
8.975940	500.489665	10.674419
8.948760	509.730975	10.679437
8.970196	500.069234	10.684455
9.073163	505.681714	10.689472
9.166121	503.218763	10.694490
8.909824	488.078629	10.699507
9.198663	486.813009	10.704525
8.739520	487.079793	10.709543
8.845171	490.534440	10.714560
8.985722	494.595316	10.719578
9.264296	501.242067	10.724595
9.332667	498.146976	10.729613
9.009140	479.494090	10.734631
8.636763	485.829288	10.739648
8.964139	484.431732	10.744666
9.243916	492.439647	10.749683
9.204430	491.991530	10.754701
8.817766	482.725527	10.759719
8.518870	498.066340	10.764736
8.701434	491.000535	10.769754
8.707270	497.652894	10.774771
9.102243	496.985075	10.779789
8.991665	502.059128	10.784807
9.052115	510.648375	10.789824
8.929798	508.039239	10.794842
8.929083	515.703135	10.799859
9.164637	510.486795	10.804877
9.000558	506.527324	10.809895
9.194656	511.594331	10.814912
9.026859	497.986036	10.819930
9.007844	505.361272	10.824947
9.039620	525.559476	10.829965
9.225041	528.810137	10.834983
9.377613	522.299078	10.840000
9.471703	506.977522	10.845018
9.140647	506.417970	10.850035
9.074849	505.723164	10.855053
9.077606	514.175615	10.860071
8.887196	526.870360	10.865088
9.187210	522.679595	10.870106
9.344186	549.928120	10.875123
9.470290	525.897290	10.880141
9.571228	539.995609	10.885159
9.494475	522.789814	10.890176
9.511296	522.030379	10.895194
9.144753	514.750438	10.900211
9.233680	508.843595	10.905229
9.243868	515.905994	10.910247
9.120651	527.714105	10.915264
9.483172	525.597774	10.920282
9.415782	533.683254	10.925299
9.381767	535.770492	10.930317
9.875223	540.612873	10.935335
9.279215	529.852082	10.940352
9.335245	508.207140	10.945370
9.090346	512.728004	10.950387
9.003617	525.600461	10.955405
9.583051	530.700039	10.960423
9.550075	530.258817	10.965440
9.638765	527.577118	10.970458
9.472141	527.472000	10.975475
9.437645	527.103554	10.980493
9.730791	541.597693	10.985511
9.652907	529.607882	10.990528
9.522710	511.877070	10.995546
9.564713	523.901532	11.000563
9.423498	498.669276	11.005581
9.711154	493.783837	11.010599
8.986861	504.844955	11.015616
9.754406	511.453222	11.020634
9.376866	524.334668	11.025651
9.388748	526.284028	11.030669
9.658008	517.117546	11.035687
9.788989	533.450650	11.040704
9.590748	529.993777	11.045722
9.679812	530.885393	11.050739
9.480337	530.889622	11.055757
9.929861	534.166018	11.060775
9.611809	528.546855	11.065792
9.849943	518.149123	11.070810
9.669883	510.066951	11.075827
9.375741	494.326284	11.080845
9.645697	507.026221	11.085863
9.778413	528.690750	11.090880
9.702750	513.653787	11.095898
9.562063	515.637904	11.100915
9.599994	509.317614	11.105933
9.589711	520.972829	11.110951
9.320746	531.076401	11.115968
9.540308	526.532558	11.120986
9.512243	534.885802	11.126003
9.767846	527.945485	11.131021
9.664782	533.414396	11.136039
9.451065	523.479351	11.141056
9.578174	528.170495	11.146074
9.613338	532.410382	11.151091
9.532628	540.619206	11.156109
9.740438	527.458272	11.161127
9.611637	533.399955	11.166144
9.967360	520.254832	11.171162
9.693047	533.367509	11.176179
9.573468	530.111379	11.181197
10.315589	530.672773	11.186215
9.715052	536.324073	11.191232
9.344100	532.539013	11.196250
9.527324	528.294036	11.201267
9.845895	555.523248	11.206285
10.222544	554.924388	11.211303
10.031649	569.945510	11.216320
10.152700	564.393903	11.221338
10.106428	545.576145	11.226355
9.743646	530.685020	11.231373
10.049563	536.335713	11.236391
9.507698	545.095957	11.241408
9.898510	553.283059	11.246426
10.383296	560.757319	11.251443
10.202530	550.243586	11.256461
9.875788	542.825188	11.261479
9.824498	536.067252	11.266496
10.074221	535.171708	11.271514
9.859992	529.834054	11.276531
10.052167	554.052409	11.281549
10.581815	550.541770	11.286567
10.152104	541.229114	11.291584
10.054088	528.860514	11.296602
9.998434	531.260425	11.301619
9.868762	537.566756	11.306637
10.384248	528.133536	11.311655
10.229502	533.271580	11.316672
10.262458	522.711231	11.321690
10.037631	528.335868	11.326707
9.963975	529.677428	11.331725
10.382325	531.797569	11.336743
10.165889	527.574353	11.341760
9.978341	520.967362	11.346778
10.137923	519.754885	11.351795
9.964226	527.182460	11.356813
9.984873	523.809966	11.361831
9.942439	531.967685	11.366848
10.246310	551.224171	11.371866
10.462189	551.945055	11.376883
9.815686	552.106311	11.381901
10.065666	550.185709	11.386919
10.139308	568.074998	11.391936
10.161803	567.315509	11.396954
10.634184	553.472460	11.401971
10.191435	563.278253	11.406989
10.645892	548.577889	11.412007
10.331471	555.601348	11.417024
10.228807	553.457181	11.422042
10.371016	548.005215	11.427059
10.105121	550.271102	11.432077
10.642837	549.817643	11.437095
10.480368	546.600383	11.442112
10.292583	541.306870	11.447130
9.978140	532.128785	11.452147
9.959265	532.924676	11.457165
10.573183	539.902475	11.462183
10.467510	552.823648	11.467200
10.381359	554.951191	11.472218
10.353554	552.086118	11.477235
10.365206	560.114562	11.482253
10.696896	541.679349	11.487271
10.281267	561.649424	11.492288
10.355665	553.244619	11.497306
10.519026	568.591087	11.502323
10.313204	563.247308	11.507341
10.528596	552.926034	11.512359
10.478921	553.589934	11.517376
10.524169	551.147849	11.522394
10.426477	561.846452	11.527411
10.296568	565.645206	11.532429
10.533024	563.204488	11.537447
10.388388	556.843397	11.542464
10.450882	558.196903	11.547482
10.407563	553.369583	11.552499
10.183148	563.781014	11.557517
10.250241	554.346003	11.562535
10.304362	569.658762	11.567552
10.333893	562.377902	11.572570
10.591840	567.488205	11.577587
10.589455	582.775871	11.582605
10.803043	593.017222	11.587623
10.693469	587.336031	11.592640
10.652913	565.267774	11.597658
10.801688	561.645695	11.602675
10.307443	567.019841	11.607693
10.411051	575.480852	11.612711
11.045525	589.201434	11.617728
10.704840	599.086627	11.622746
10.838200	581.573061	11.627763
10.885436	579.938671	11.632781
10.903203	565.649076	11.637799
11.001524	554.105930	11.642816
10.585684	558.157998	11.647834
11.150070	557.730933	11.652851
10.727734	561.119429	11.657869
10.877662	554.795965	11.662887
10.707942	554.923404	11.667904
10.590295	558.607944	11.672922
10.878924	549.067737	11.677939
10.677136	557.986811	11.682957
10.586025	569.540086	11.687975
10.693349	578.102632	11.692992
10.807700	587.797780	11.698010
11.361339	586.463398	11.703027
10.699330	578.596046	11.708045
10.678841	563.372488	11.713063
10.851472	571.678120	11.718080
10.926149	579.723320	11.723098
10.984381	581.166788	11.728115
10.880235	577.129789	11.733133
11.101808	580.048069	11.738151
11.062220	600.766343	11.743168
10.481575	588.052918	11.748186
11.141532	585.766780	11.753203
11.059296	586.736403	11.758221
11.139389	585.938266	11.763239
11.175316	592.206625	11.768256
11.052558	575.301532	11.773274
11.140617	562.434619	11.778291
10.651907	560.693359	11.783309
10.763356	565.552033	11.788327
10.522902	583.074619	11.793344
10.251448	586.440056	11.798362
11.100405	587.499358	11.803379
11.000908	593.291955	11.808397
11.236532	579.377791	11.813415
11.150158	580.569909	11.818432
10.714186	597.614772	11.823450
11.113725	590.672291	11.828467
11.048738	599.890085	11.833485
11.350603	592.581527	11.838503
11.308167	588.007844	11.843520
10.926445	588.756238	11.848538
10.865012	591.953824	11.853555
10.931458	599.417327	11.858573
11.210002	609.614496	11.863591
11.468978	624.311864	11.868608
11.244507	614.750127	11.873626
11.551034	590.508310	11.878643
11.107822	589.232673	11.883661
11.401371	591.977376	11.888679
11.291572	583.770287	11.893696
10.898274	597.283913	11.898714
11.429407	598.849594	11.903731
11.165805	596.366234	11.908749
11.207149	596.335980	11.913767
11.390965	606.161467	11.918784
11.388472	622.886933	11.923802
11.712143	615.967902	11.928819
11.522173	599.657842	11.933837
11.469289	591.493992	11.938855
11.429563	586.633495	11.943872
11.034777	588.073789	11.948890
11.376200	593.735562	11.953907
11.037358	599.873172	11.958925
11.213353	614.224365	11.963943
11.716189	614.094724	11.968960
11.351363	620.124254	11.973978
11.379003	616.662312	11.978995
11.535227	616.719159	11.984013
11.580037	612.393015	11.989031
11.656558	621.146765	11.994048
11.492576	626.268751	11.999066
11.472346	617.656162	12.004083
11.559745	619.478606	12.009101
11.378706	614.151183	12.014119
11.755506	620.970304	12.019136
11.412828	623.367965	12.024154
11.506718	620.132238	12.029171
11.736247	609.404625	12.034189
11.382202	622.658090	12.039207
11.655939	615.944028	12.044224
11.685193	618.952452	12.049242
11.880704	627.931186	12.054259
11.848294	617.080347	12.059277
11.774938	612.872236	12.064295
11.661691	593.333920	12.069312
11.255897	597.764292	12.074330
11.474231	609.728978	12.079347
11.527171	609.639437	12.084365
11.685555	618.521661	12.089383
12.207318	619.323769	12.094400
11.700358	622.944827	12.099418
11.762788	613.252624	12.104435
11.924775	625.907323	12.109453
11.925772	623.973240	12.114471
11.987387	613.924933	12.119488
11.839441	605.255713	12.124506
11.430667	594.142830	12.129523
11.697859	592.569711	12.134541
11.754121	610.051659	12.139559
11.901487	613.342086	12.144576
11.596066	620.734298	12.149594
11.853154	624.602064	12.154611
11.926307	617.764777	12.159629
11.903829	617.333626	12.164647
12.053653	616.262691	12.169664
11.708832	629.228761	12.174682
11.722489	620.847735	12.179699
11.914250	623.411267	12.184717
11.553672	615.681747	12.189735
11.792749	612.454898	12.194752
11.643849	622.103921	12.199770
11.855319	614.544490	12.204787
11.664261	615.482697	12.209805
11.605898	617.848036	12.214823
11.968155	617.413336	12.219840
11.587159	628.520451	12.224858
11.790519	641.206706	12.229875
11.915676	647.265100	12.234893
12.129029	642.902435	12.239911
12.270025	650.750032	12.244928
12.320858	647.486480	12.249946
12.216900	651.441568	12.254963
12.271448	654.009870	12.259981
12.249299	633.978775	12.264999
12.257740	620.129375	12.270016
11.983108	631.173155	12.275034
12.421678	627.496086	12.280051
12.052220	630.672055	12.285069
11.908659	633.187673	12.290087
12.405650	631.092801	12.295104
11.972220	631.864699	12.300122
11.913754	628.656214	12.305139
12.122829	649.875102	12.310157
12.164764	665.187804	12.315175
12.490172	659.141546	12.320192
12.170549	663.854004	12.325210
12.687229	651.030243	12.330227
12.518059	653.823277	12.335245
12.154456	638.894690	12.340263
12.242260	629.599198	12.345280
12.116707	642.396293	12.350298
12.223900	644.472511	12.355315
12.448671	649.552799	12.360333
12.238473	650.517297	12.365351
12.275685	657.705392	12.370368
12.531941	665.062770	12.375386
12.318028	663.061261	12.380403
12.401346	655.469060	12.385421
12.256330	659.551387	12.390439
12.392752	650.451849	12.395456
12.482795	660.685221	12.400474
12.299729	659.382432	12.405491
12.549454	666.129970	12.410509
12.093192	672.207302	12.415527
12.242240	657.348974	12.420544
12.067006	653.094804	12.425562
12.471609	651.537253	12.430579
12.456817	652.195294	12.435597
12.499968	657.069417	12.440615
12.512374	656.952032	12.445632
12.162750	656.818305	12.450650
12.140088	652.528098	12.455667
12.471391	671.296327	12.460685
12.393430	691.894118	12.465703
12.625615	673.642487	12.470720
12.439536	690.276731	12.475738
12.511355	684.186754	12.480755
12.890411	680.906154	12.485773
12.667690	680.150967	12.490791
13.151886	679.935739	12.495808
12.953017	681.562822	12.500826
12.494846	665.061817	12.505843
12.725852	659.739306	12.510861
12.572924	654.160612	12.515879
12.560998	660.983074	12.520896
12.266116	669.596096	12.525914
12.427557	688.491218	12.530931
12.825174	687.332585	12.535949
12.760461	687.538915	12.540967
12.939979	680.637575	12.545984
12.996965	689.382586	12.551002
12.625254	687.692536	12.556019
12.841330	683.341809	12.561037
12.426989	685.753585	12.566055
12.806630	683.814394	12.571072
12.868632	691.009429	12.576090
12.584531	690.608815	12.581107
12.995828	689.099358	12.586125
12.793166	683.102566	12.591143
12.812785	680.652100	12.596160
12.427548	690.223803	12.601178
12.531911	677.487247	12.606195
13.015974	697.211003	12.611213
12.890045	703.571892	12.616231
13.071584	701.887445	12.621248
13.004954	689.398194	12.626266
12.998392	693.505477	12.631283
13.220315	685.709284	12.636301
12.865997	684.089970	12.641319
13.142855	677.744299	12.646336
13.275848	679.253756	12.651354
12.868713	681.253189	12.656371
12.846879	687.805102	12.661389
13.240507	699.377467	12.666407
12.922382	686.217890	12.671424
13.302352	692.696321	12.676442
13.240518	698.091461	12.681459
13.183786	683.021879	12.686477
12.841167	692.647947	12.691495
13.212523	700.717105	12.696512
13.378207	706.180144	12.701530
13.241762	700.776632	12.706547
13.517281	685.636791	12.711565
13.195882	684.442082	12.716583
13.313153	677.935413	12.721600
12.967405	675.429202	12.726618
13.147798	668.476551	12.731635
13.168844	673.732614	12.736653
13.137193	697.387595	12.741671
13.178651	694.640653	12.746688
13.612177	706.888207	12.751706
13.549982	702.323857	12.756723
13.336285	682.482397	12.761741
13.342807	687.777669	12.766759
12.992426	676.372546	12.771776
13.174438	701.350657	12.776794
13.199255	715.539065	12.781811
13.246455	711.412661	12.786829
13.111813	719.833314	12.791847
13.126897	710.563075	12.796864
13.213145	710.628928	12.801882
13.120965	709.790563	12.806899
13.452597	708.962662	12.811917
13.608117	719.002015	12.816935
13.335910	713.314095	12.821952
13.566639	702.045955	12.826970
13.462987	700.759759	12.831987
13.615733	702.585979	12.837005
13.344381	716.615688	12.842023
13.612285	711.740333	12.847040
13.664493	714.671372	12.852058
13.578585	700.828241	12.857075
13.540522	705.863806	12.862093
13.116674	713.763839	12.867111
13.337855	708.684233	12.872128
13.691145	713.880879	12.877146
13.951175	731.443446	12.882163
14.038992	717.033492	12.887181
13.595339	713.870141	12.892199
13.773147	710.515723	12.897216
13.503877	714.067902	12.902234
13.777533	713.529652	12.907251
13.804176	702.348182	12.912269
13.743417	707.387105	12.917287
13.776858	710.736530	12.922304
13.736566	700.048522	12.927322
13.060839	721.229895	12.932339
14.133271	715.452033	12.937357
13.711538	730.333238	12.942375
13.982517	738.309375	12.947392
14.367586	726.559292	12.952410
13.683199	720.106747	12.957427
13.656273	706.995669	12.962445
13.658393	718.323939	12.967463
13.766934	721.224612	12.972480
14.302497	734.238856	12.977498
13.818710	737.123260	12.982515
13.902589	712.762066	12.987533
13.862902	726.943627	12.992551
14.162732	735.142516	12.997568
13.982280	717.141669	13.002586
13.815436	706.857182	13.007603
13.840224	707.717902	13.012621
13.904775	726.969183	13.017639
13.873352	735.633374	13.022656
13.928251	744.994999	13.027674
13.853245	743.922730	13.032691
14.337485	743.007610	13.037709
14.078952	729.016434	13.042727
14.138912	728.479448	13.047744
14.190635	734.057573	13.052762
14.048852	752.659435	13.057779
14.172416	731.843432	13.062797
13.705933	735.890727	13.067815
13.993378	743.750976	13.072832
14.216961	731.850832	13.077850
14.038481	745.882737	13.082867
14.009010	745.858281	13.087885
13.974176	740.590302	13.092903
13.985184	736.540923	13.097920
13.931247	725.513083	13.102938
13.883233	739.259096	13.107955
14.079438	751.010951	13.112973
14.224639	759.494418	13.117991
14.237657	767.044378	13.123008
14.406591	768.541015	13.128026
14.426360	776.369543	13.133043
14.403868	769.591688	13.138061
14.401185	772.916786	13.143079
14.543990	769.749015	13.148096
14.931092	759.376693	13.153114
14.678617	740.980896	13.158131
14.567062	733.521433	13.163149
14.463013	736.338755	13.168167
14.464399	742.730580	13.173184
14.530444	724.378018	13.178202
14.397810	739.942637	13.183219
14.692323	732.639066	13.188237
14.741404	732.986408	13.193255
14.458075	743.192377	13.198272
14.541454	730.415158	13.203290
14.512461	734.442708	13.208307
14.685425	730.470290	13.213325
14.490411	729.755396	13.218343
14.393805	729.573756	13.223360
14.605031	724.935087	13.228378
14.140781	745.971329	13.233395
14.182277	731.705608	13.238413
14.323327	735.335041	13.243431
13.965208	748.705016	13.248448
14.778374	753.716447	13.253466
14.524092	771.168807	13.258483
14.578431	764.823067	13.263501
14.574769	766.446832	13.268519
14.641807	780.020351	13.273536
14.698697	766.625533	13.278554
14.892754	778.449209	13.283571
14.621401	781.969864	13.288589
14.643374	768.312354	13.293607
14.689652	773.862462	13.298624
14.727282	765.771146	13.303642
14.525248	770.599418	13.308659
14.645316	771.636885	13.313677
14.785571	777.109072	13.318695
14.359572	765.022004	13.323712
14.963263	775.100897	13.328730
15.079152	795.205844	13.333747
15.028870	784.687905	13.338765
14.923467	778.094979	13.343783
14.666948	785.247435	13.348800
15.023891	777.591456	13.353818
15.118817	792.527675	13.358835
14.916721	770.069843	13.363853
15.174234	776.165462	13.368871
14.826744	782.660224	13.373888
15.244151	777.313168	13.378906
14.934898	772.355246	13.383923
15.070023	779.550639	13.388941
15.250143	776.197596	13.393959
14.862662	782.156929	13.398976
15.197092	788.555736	13.403994
14.920326	788.180083	13.409011
15.275755	793.643092	13.414029
15.509117	781.254759	13.419047
14.896554	784.087629	13.424064
15.277254	780.233011	13.429082
14.915795	777.010599	13.434099
14.986237	796.251349	13.439117
15.179344	788.184124	13.444135
15.478365	795.064101	13.449152
15.545052	800.255981	13.454170
15.578906	797.886989	13.459187
15.290291	790.629171	13.464205
14.952035	767.850985	13.469223
15.386836	782.313775	13.474240
15.537377	782.071414	13.479258
15.403457	779.524670	13.484275
15.238937	772.403612	13.489293
15.387948	771.613758	13.494311
15.315657	772.794805	13.499328
15.377453	762.791344	13.504346
15.185107	774.271457	13.509363
15.168819	792.477493	13.514381
15.755793	802.420016	13.519399
15.646410	791.668767	13.524416
15.362183	772.351558	13.529434
15.348562	776.009710	13.534451
15.693933	792.257668	13.539469
15.688833	787.781283	13.544487
15.129650	778.821024	13.549504
15.501536	781.636858	13.554522
15.527554	796.234131	13.559539
15.354990	794.614292	13.564557
15.770257	798.559784	13.569575
15.391112	795.390873	13.574592
15.535205	790.908728	13.579610
15.605357	801.674922	13.584627
15.578419	805.771628	13.589645
15.701688	797.821827	13.594663
15.434691	796.332338	13.599680
15.790085	799.304813	13.604698
15.386611	797.657394	13.609715
15.686899	804.527915	13.614733
15.827438	791.742184	13.619751
15.406913	798.418679	13.624768
15.740663	798.207450	13.629786
15.673636	803.192724	13.634803
15.487208	800.929807	13.639821
15.681377	793.164520	13.644839
15.414313	809.607191	13.649856
15.970590	810.982747	13.654874
16.129831	821.436840	13.659891
15.570413	830.340477	13.664909
15.723440	819.645042	13.669927
15.348331	847.928131	13.674944
15.732989	826.935803	13.679962
15.948147	828.440357	13.684979
15.887314	835.501059	13.689997
16.239024	830.047341	13.695015
15.535564	833.697671	13.700032
15.951592	839.993856	13.705050
15.590253	835.950873	13.710067
16.014043	836.852340	13.715085
15.931742	825.820456	13.720103
15.720308	836.610966	13.725120
16.051750	841.171998	13.730138
16.380031	854.978746	13.735155
16.070874	854.967050	13.740173
15.954814	830.771956	13.745191
15.957735	843.752285	13.750208
16.215401	851.211472	13.755226
16.151114	870.191159	13.760243
16.152714	859.065476	13.765261
16.238353	850.824079	13.770279
15.982114	868.692357	13.775296
16.039534	860.863034	13.780314
16.073058	864.724209	13.785331
16.099974	868.409537	13.790349
16.474102	868.148924	13.795367
16.267794	855.572401	13.800384
16.311883	862.528980	13.805402
16.387609	864.213640	13.810419
16.435909	864.153108	13.815437
16.288251	864.910071	13.820455
16.366185	865.795476	13.825472
16.664510	863.864387	13.830490
16.887716	864.319157	13.835507
16.651314	861.044964	13.840525
16.481947	853.942580	13.845543
16.050950	865.023093	13.850560
16.207596	857.441112	13.855578
16.864739	859.449115	13.860595
16.508298	864.220268	13.865613
16.910181	856.928812	13.870631
16.539935	859.374660	13.875648
16.429303	857.519418	13.880666
16.472687	862.042442	13.885683
16.327537	858.681921	13.890701
16.185280	867.174964	13.895719
16.086526	861.649831	13.900736
16.050385	851.673518	13.905754
16.240126	860.807254	13.910771
15.997934	881.587335	13.915789
16.641173	878.236664	13.920807
16.294194	890.320082	13.925824
16.407239	879.714467	13.930842
16.479609	887.437917	13.935859
16.563792	897.003030	13.940877
16.817437	897.821218	13.945895
16.373154	895.282246	13.950912
16.685966	896.871244	13.955930
16.757834	905.673753	13.960947
16.871064	914.845751	13.965965
17.012438	908.436562	13.970983
16.832056	924.709543	13.976000
16.810451	914.358797	13.981018
16.920986	918.380855	13.986035
17.043732	909.950251	13.991053
17.245414	918.185533	13.996071
16.801831	908.535332	14.001088
17.223171	916.655783	14.006106
17.290054	901.810600	14.011123
16.968486	896.722803	14.016141
17.273348	887.435079	14.021159
17.335619	897.090021	14.026176
16.666576	895.388263	14.031194
17.199144	886.528587	14.036211
16.960186	886.169712	14.041229
17.225286	889.691295	14.046247
17.377834	895.642717	14.051264
17.023849	893.187824	14.056282
17.108769	884.762107	14.061299
16.728116	891.512552	14.066317
17.266332	892.242579	14.071335
17.288423	884.774342	14.076352
17.438640	892.665413	14.081370
17.538695	893.464304	14.086387
17.361258	888.719761	14.091405
17.613127	893.183936	14.096423
17.371895	885.446465	14.101440
17.743127	889.578955	14.106458
17.785979	890.132613	14.111475
17.278130	889.981336	14.116493
17.409744	881.167255	14.121511
17.247051	896.745462	14.126528
17.292286	892.733490	14.131546
17.363724	889.770569	14.136563
17.367663	901.845408	14.141581
17.384881	892.845138	14.146599
17.129569	886.064570	14.151616
17.094955	893.196742	14.156634
16.942504	895.803227	14.161651
17.206156	892.284804	14.166669
17.556804	907.545748	14.171687
17.833430	917.800419	14.176704
17.832478	914.999432	14.181722
17.375874	900.879044	14.186739
17.164870	902.101918	14.191757
17.485854	908.185132	14.196775
17.368765	906.878505	14.201792
17.443748	917.329660	14.206810
17.756826	906.739586	14.211827
17.197093	914.521055	14.216845
17.602130	912.641410	14.221863
17.603653	918.507579	14.226880
17.408822	926.744423	14.231898
17.482854	912.529448	14.236915
17.226976	919.342148	14.241933
17.788841	937.410301	14.246951
17.626047	940.723908	14.251968
17.690213	944.642628	14.256986
17.657841	946.783874	14.262003
17.504121	955.451472	14.267021
17.566106	948.347224	14.272039
17.765148	951.667958	14.277056
17.668349	950.183591	14.282074
18.017083	943.195321	14.287091
17.597380	948.300921	14.292109
17.996988	943.823941	14.297127
17.957420	954.639865	14.302144
17.653276	945.117560	14.307162
17.788583	950.449113	14.312179
17.755914	968.006193	14.317197
18.245241	973.408760	14.322215
18.454906	973.689223	14.327232
18.248284	964.767627	14.332250
17.920816	954.607928	14.337267
18.054123	976.978198	14.342285
18.155028	972.350601	14.347303
18.249729	984.764784	14.352320
18.045749	970.248899	14.357338
18.231544	972.629842	14.362355
18.467503	984.010597	14.367373
18.517922	975.009123	14.372391
18.278311	963.857487	14.377408
18.132899	948.157318	14.382426
18.439249	940.119915	14.387443
18.144573	946.497373	14.392461
18.451750	950.897709	14.397479
18.320546	950.919194	14.402496
18.053555	952.598500	14.407514
18.515013	955.973887	14.412531
18.402315	984.945445	14.417549
18.509656	974.069489	14.422567
18.476835	976.891617	14.427584
18.566113	980.011434	14.432602
18.579581	971.599445	14.437619
18.467086	951.551572	14.442637
18.329293	948.503154	14.447655
18.350459	953.261534	14.452672
18.507826	976.109644	14.457690
18.864325	968.182425	14.462707
18.502432	977.067873	14.467725
18.584239	976.863241	14.472743
18.675687	987.201700	14.477760
18.532324	981.766954	14.482778
18.640419	975.160314	14.487795
18.400671	967.718969	14.492813
18.587579	975.736480	14.497831
18.653388	978.119341	14.502848
18.266102	984.728622	14.507866
18.651230	976.722270	14.512883
18.448040	982.659098	14.517901
18.749191	977.407552	14.522919
18.951881	972.656260	14.527936
18.394008	981.115897	14.532954
18.616882	976.027264	14.537971
18.506969	989.954570	14.542989
18.744240	982.475329	14.548007
18.837023	994.293469	14.553024
18.813089	1002.116343	14.558042
18.888040	1017.392645	14.563059
19.117935	1016.312485	14.568077
18.880159	1017.343561	14.573095
19.315858	1007.219107	14.578112
18.771042	1007.036147	14.583130
19.154558	1003.068034	14.588147
18.909849	1008.872777	14.593165
19.043348	1002.298339	14.598183
19.046959	994.812436	14.603200
18.833347	1006.032691	14.608218
18.667043	1007.341283	14.613235
18.974926	1015.767305	14.618253
18.877857	1012.462181	14.623271
19.241602	1009.476913	14.628288
18.971866	1021.044200	14.633306
18.934848	1013.351647	14.638323
19.403274	1004.900279	14.643341
19.231535	1009.346510	14.648359
19.210411	1010.047733	14.653376
19.163921	1017.660987	14.658394
18.841884	1014.551087	14.663411
18.972280	1012.043292	14.668429
19.147972	1031.323430	14.673447
19.428469	1026.802733	14.678464
19.315901	1046.981190	14.683482
19.405195	1044.346933	14.688499
19.344196	1033.509381	14.693517
19.284627	1037.698733	14.698535
19.384001	1030.933691	14.703552
19.405226	1030.508001	14.708570
19.963015	1020.697763	14.713587
19.562486	1040.362462	14.718605
19.457493	1042.057717	14.723623
19.458487	1037.582811	14.728640
19.532079	1038.362267	14.733658
19.612241	1038.739515	14.738675
19.299894	1042.596875	14.743693
19.698029	1041.949081	14.748711
19.696350	1036.747952	14.753728
19.474152	1044.102305	14.758746
19.899045	1037.934554	14.763763
20.040098	1024.692706	14.768781
19.270555	1043.121924	14.773799
19.620365	1036.098597	14.778816
19.454089	1043.412021	14.783834
19.973335	1034.054732	14.788851
19.901638	1037.198604	14.793869
19.738453	1026.456279	14.798887
19.777903	1034.711346	14.803904
19.419385	1049.305681	14.808922
19.943395	1042.598987	14.813939
19.687345	1047.756501	14.818957
19.597888	1036.420180	14.823975
20.045084	1030.845903	14.828992
19.582553	1040.023173	14.834010
19.665221	1042.652632	14.839027
19.836097	1069.550815	14.844045
19.958265	1075.689191	14.849063
19.947823	1074.850880	14.854080
19.827419	1074.107697	14.859098
20.064947	1066.877747	14.864115
20.273151	1070.648502	14.869133
20.086197	1074.905365	14.874151
20.192240	1071.091536	14.879168
19.894928	1070.950537	14.884186
19.917794	1074.088039	14.889203
20.174149	1076.537445	14.894221
19.882920	1070.364614	14.899239
20.241503	1072.975053	14.904256
19.968186	1077.230245	14.909274
20.239761	1072.220331	14.914291
20.141644	1077.188985	14.919309
20.062370	1080.668124	14.924327
19.952428	1076.808304	14.929344
20.219255	1077.082866	14.934362
20.595682	1086.723802	14.939379
20.682781	1098.877953	14.944397
20.560429	1097.902447	14.949415
20.222342	1081.537427	14.954432
20.084410	1082.517761	14.959450
20.476375	1099.818430	14.964467
20.448143	1095.687068	14.969485
20.093884	1100.324094	14.974503
20.401155	1096.946230	14.979520
20.750287	1103.054197	14.984538
20.226859	1107.073012	14.989555
20.358237	1101.167685	14.994573
20.476494	1101.771087	14.999591
20.517801	1104.348147	15.004608
20.468450	1107.062612	15.009626
20.922573	1099.594324	15.014643
20.649546	1100.543448	15.019661
20.238563	1097.202594	15.024679
20.394375	1096.302168	15.029696
20.477702	1108.121761	15.034714
20.815687	1136.531008	15.039731
20.852662	1135.165836	15.044749
20.923268	1144.290888	15.049767
21.213329	1133.243504	15.054784
20.752372	1117.426629	15.059802
20.703032	1130.950210	15.064819
20.925326	1129.292443	15.069837
20.889969	1137.230643	15.074855
20.977378	1142.229083	15.079872
20.731459	1139.674807	15.084890
20.591176	1129.570465	15.089907
20.390012	1136.254353	15.094925
20.395599	1140.738238	15.099943
20.759305	1137.499248	15.104960
20.608887	1150.073739	15.109978
21.096173	1147.120188	15.114995
21.390387	1164.801796	15.120013
20.909115	1172.442099	15.125031
21.220323	1176.155314	15.130048
20.861045	1176.614237	15.135066
21.129757	1168.939579	15.140083
21.376547	1157.547998	15.145101
20.793381	1170.252473	15.150119
21.261125	1165.070368	15.155136
20.920708	1167.197203	15.160154
21.213423	1184.921203	15.165171
21.316771	1158.129254	15.170189
21.236666	1181.969732	15.175207
21.342166	1165.608082	15.180224
21.310169	1169.728749	15.185242
21.104433	1165.827264	15.190259
21.136243	1161.144699	15.195277
21.512309	1155.416800	15.200295
21.495533	1161.309311	15.205312
20.915784	1162.785239	15.210330
21.152404	1186.860749	15.215347
21.420300	1195.388542	15.220365
21.235669	1202.173650	15.225383
21.519161	1190.572070	15.230400
21.511356	1195.606535	15.235418
21.412183	1200.581307	15.240435
22.259522	1204.811560	15.245453
22.090022	1200.449021	15.250471
21.926743	1200.034527	15.255488
22.048403	1190.707024	15.260506
21.728296	1181.799331	15.265523
22.177324	1169.001675	15.270541
21.821580	1177.156006	15.275559
22.070325	1166.625591	15.280576
21.957281	1171.602843	15.285594
21.751317	1165.817599	15.290611
22.219203	1162.651729	15.295629
21.838185	1157.204232	15.300647
22.153092	1163.911695	15.305664
22.326614	1156.238996	15.310682
22.169546	1172.839049	15.315699
22.470104	1167.540102	15.320717
21.811307	1153.785722	15.325735
21.753807	1146.242334	15.330752
21.921360	1151.752461	15.335770
21.617628	1165.792258	15.340787
21.843567	1155.430360	15.345805
21.764227	1159.326400	15.350823
21.826298	1160.371509	15.355840
21.692246	1174.575374	15.360858
21.564828	1178.089849	15.365875
21.591869	1183.178583	15.370893
21.485402	1192.837778	15.375911
21.566788	1198.047636	15.380928
21.641675	1207.691436	15.385946
21.735687	1218.605140	15.390963
21.976761	1226.383941	15.395981
21.944780	1233.981914	15.400999
22.150026	1229.501936	15.406016
22.386716	1226.412640	15.411034
22.099829	1233.711443	15.416051
22.242523	1236.453046	15.421069
21.914583	1234.000682	15.426087
21.868043	1234.683874	15.431104
22.186949	1246.157598	15.436122
22.424081	1261.182567	15.441139
22.594643	1255.448243	15.446157
22.772318	1253.584085	15.451175
22.738774	1264.504531	15.456192
22.743296	1249.270553	15.461210
22.781411	1249.361880	15.466227
23.165103	1248.959937	15.471245
22.743532	1230.131716	15.476263
22.631829	1216.839949	15.481280
22.725311	1212.319594	15.486298
22.385442	1224.119852	15.491315
22.665095	1218.973535	15.496333
22.696512	1222.527512	15.501351
22.848974	1230.846282	15.506368
22.704639	1227.515856	15.511386
22.456914	1238.519113	15.516403
22.813006	1247.459666	15.521421
22.733911	1257.351945	15.526439
22.835208	1256.592981	15.531456
22.836538	1245.239339	15.536474
23.093425	1253.894952	15.541491
23.233883	1249.835857	15.546509
23.152977	1260.880844	15.551527
22.899273	1251.333284	15.556544
23.162557	1252.523865	15.561562
22.986357	1250.034417	15.566579
23.219418	1249.259977	15.571597
23.084949	1252.631953	15.576615
23.190419	1255.100614	15.581632
23.052517	1234.700516	15.586650
22.962548	1242.284654	15.591667
23.026097	1249.049437	15.596685
23.169068	1256.784236	15.601703
23.242473	1257.851295	15.606720
23.362064	1248.158399	15.611738
23.476945	1263.432086	15.616755
23.491368	1243.701595	15.621773
23.441016	1233.923420	15.626791
23.222098	1224.521682	15.631808
23.380226	1221.707736	15.636826
23.251670	1237.770344	15.641843
22.999031	1239.980112	15.646861
22.930959	1245.589044	15.651879
23.244260	1249.639091	15.656896
23.253989	1246.254269	15.661914
23.111875	1259.298871	15.666931
23.233266	1252.609808	15.671949
22.960973	1258.808521	15.676967
23.063200	1263.008397	15.681984
23.336048	1264.354268	15.687002
23.285522	1278.400941	15.692019
23.558403	1274.285709	15.697037
23.720937	1282.944727	15.702055
23.425034	1283.844892	15.707072
23.891354	1282.422535	15.712090
23.471191	1282.789369	15.717107
23.747907	1277.321119	15.722125
23.595267	1279.251410	15.727143
23.985999	1280.921262	15.732160
23.754229	1283.347637	15.737178
23.885221	1284.080814	15.742195
24.125580	1282.758388	15.747213
23.764848	1283.181534	15.752231
24.006181	1274.970671	15.757248
24.235521	1268.374180	15.762266
23.717315	1282.294624	15.767283
23.764797	1274.562980	15.772301
23.904990	1283.642172	15.777319
23.692596	1279.954525	15.782336
23.895116	1288.840373	15.787354
23.724370	1302.283983	15.792371
24.437160	1304.076382	15.797389
24.131737	1300.932185	15.802407
24.021021	1319.572701	15.807424
24.337951	1306.983941	15.812442
24.530931	1311.541620	15.817459
24.360402	1295.680898	15.822477
23.996281	1297.100146	15.827495
23.955428	1304.767721	15.832512
24.346921	1319.931392	15.837530
24.196702	1308.958804	15.842547
24.494076	1315.174412	15.847565
24.338108	1313.230359	15.852583
24.302965	1303.332122	15.857600
24.482798	1308.070099	15.862618
24.426838	1316.020259	15.867635
24.245714	1312.075502	15.872653
24.426766	1307.004890	15.877671
24.535016	1320.865148	15.882688
24.735045	1303.281585	15.887706
24.683030	1317.354126	15.892723
24.541756	1315.751105	15.897741
24.768679	1312.181184	15.902759
24.456116	1312.213349	15.907776
24.364290	1304.142947	15.912794
24.234770	1320.391209	15.917811
24.518265	1313.250583	15.922829
24.523394	1311.105128	15.927847
24.380831	1316.231183	15.932864
24.704407	1307.263303	15.937882
24.644653	1304.407404	15.942899
24.726120	1304.721262	15.947917
24.210109	1316.269434	15.952935
24.250694	1342.546202	15.957952
24.911642	1342.021285	15.962970
24.849215	1347.353568	15.967987
25.076606	1348.487498	15.973005
25.159778	1339.214488	15.978023
24.894678	1338.648924	15.983040
24.968300	1339.069184	15.988058
25.103851	1337.353494	15.993075
25.147913	1334.484370	15.998093
25.348167	1335.982975	16.003111
25.228991	1347.063871	16.008128
25.265964	1324.052405	16.013146
25.157716	1347.868464	16.018163
25.033421	1343.782040	16.023181
25.286383	1338.966825	16.028199
25.083333	1339.904005	16.033216
25.675936	1335.955973	16.038234
25.487792	1342.643704	16.043251
25.228840	1346.772989	16.048269
25.280026	1327.697256	16.053287
25.283187	1337.449632	16.058304
25.423544	1334.820862	16.063322
25.199800	1338.774860	16.068339
25.208660	1334.797127	16.073357
25.092912	1319.989595	16.078375
25.042582	1342.971771	16.083392
25.794680	1327.242572	16.088410
25.341051	1333.098297	16.093427
25.550394	1335.471273	16.098445
25.484418	1328.987526	16.103463
25.352086	1330.074022	16.108480
25.866844	1355.242271	16.113498
26.012589	1364.828404	16.118515
26.149959	1360.357637	16.123533
26.248844	1332.370996	16.128551
26.033730	1339.486554	16.133568
26.020702	1327.918322	16.138586
25.862907	1319.506495	16.143603
25.826144	1320.658684	16.148621
25.857871	1326.927446	16.153639
25.705294	1333.215644	16.158656
26.251106	1319.932441	16.163674
26.248417	1322.946281	16.168691
25.784145	1316.908033	16.173709
25.810865	1325.668446	16.178727
25.924437	1329.555284	16.183744
25.852563	1330.734730	16.188762
25.691283	1332.696963	16.193779
26.020041	1327.980235	16.198797
26.071090	1332.355889	16.203815
25.922960	1339.865838	16.208832
26.030007	1336.763499	16.213850
26.071682	1324.139118	16.218867
25.852105	1325.600419	16.223885
26.087413	1344.351676	16.228903
26.045866	1361.984678	16.233920
26.053376	1368.968591	16.238938
26.032742	1372.745547	16.243955
25.895278	1371.735911	16.248973
26.435752	1365.586722	16.253991
25.927305	1372.669479	16.259008
26.039997	1368.657258	16.264026
26.238025	1364.932868	16.269043
26.247267	1380.116858	16.274061
26.498492	1384.940687	16.279079
26.522791	1388.137655	16.284096
26.420687	1405.508110	16.289114
26.643408	1392.389048	16.294131
26.337735	1398.532121	16.299149
26.516168	1393.931542	16.304167
26.612548	1385.024977	16.309184
26.515852	1386.559469	16.314202
26.482575	1393.573752	16.319219
25.990811	1385.569003	16.324237
26.295468	1387.759130	16.329255
26.336690	1397.790062	16.334272
26.938166	1406.831678	16.339290
27.074945	1411.854524	16.344307
26.924127	1411.654671	16.349325
26.941205	1417.513538	16.354343
26.709064	1428.776527	16.359360
27.025283	1426.504461	16.364378
27.118627	1422.197626	16.369395
26.726409	1414.280336	16.374413
27.206695	1408.267439	16.379431
27.129415	1431.326632	16.384448
27.088661	1411.780023	16.389466
27.084153	1418.823811	16.394483
26.917642	1415.019901	16.399501
27.229021	1425.495715	16.404519
27.265993	1415.221951	16.409536
27.263861	1412.933802	16.414554
27.170772	1403.272608	16.419571
26.987498	1417.226199	16.424589
27.221643	1418.957568	16.429607
27.168329	1417.167581	16.434624
27.376743	1420.950985	16.439642
27.748235	1408.802284	16.444659
27.225277	1415.579031	16.449677
27.456301	1407.392436	16.454695
27.238073	1417.313714	16.459712
27.364136	1419.788250	16.464730
27.242967	1408.097490	16.469747
26.875105	1413.265138	16.474765
27.226357	1413.632633	16.479783
27.462445	1426.110805	16.484800
27.339710	1446.403654	16.489818
27.468573	1447.500533	16.494835
27.679169	1447.024250	16.499853
28.102958	1426.003387	16.504871
28.229936	1432.187168	16.509888
28.214758	1428.015376	16.514906
28.299056	1416.400289	16.519923
28.201993	1415.307409	16.524941
28.097816	1411.938027	16.529959
28.179539	1407.726805	16.534976
28.177880	1408.543515	16.539994
28.281195	1393.587522	16.545011
27.840222	1397.451069	16.550029
28.379946	1406.455257	16.555047
28.137092	1414.842404	16.560064
27.976524	1407.125982	16.565082
28.082099	1398.934535	16.570099
27.437149	1411.926351	16.575117
28.063374	1404.490297	16.580135
28.077057	1411.672397	16.585152
28.110562	1405.058610	16.590170
28.006773	1411.928076	16.595187
27.691524	1405.511667	16.600205
27.950002	1401.260413	16.605223
28.024693	1401.973966	16.610240
28.159500	1412.851542	16.615258
28.507192	1409.382494	16.620275
28.073851	1407.412422	16.625293
28.192332	1406.092018	16.630311
28.223329	1421.427552	16.635328
28.442198	1429.751203	16.640346
28.318157	1440.559185	16.645363
28.486121	1437.177500	16.650381
28.580482	1432.922849	16.655399
28.619518	1430.028557	16.660416
28.270079	1436.251112	16.665434
28.339423	1439.653023	16.670451
28.327123	1444.174790	16.675469
28.635261	1436.322443	16.680487
28.376733	1428.339161	16.685504
28.402602	1434.887642	16.690522
28.593670	1432.797457	16.695539
28.294291	1458.690694	16.700557
28.275968	1455.146112	16.705575
28.526053	1459.472377	16.710592
28.581163	1464.701234	16.715610
28.704438	1466.943981	16.720627
28.343944	1476.543768	16.725645
28.728874	1469.509325	16.730663
28.645823	1484.755514	16.735680
28.854091	1490.354889	16.740698
29.108593	1487.355501	16.745715
28.957462	1492.721388	16.750733
29.172218	1492.949846	16.755751
29.416568	1491.640521	16.760768
29.162803	1490.129289	16.765786
29.303156	1485.601110	16.770803
28.940015	1483.927266	16.775821
29.168783	1479.480727	16.780839
29.275966	1492.414259	16.785856
29.209913	1496.552056	16.790874
29.591028	1486.386711	16.795891
29.548205	1488.757881	16.800909
29.471285	1479.112863	16.805927
29.700806	1479.259362	16.810944
29.812012	1487.053655	16.815962
29.865016	1492.288970	16.820979
29.343400	1480.465533	16.825997
29.642171	1477.574172	16.831015
29.755800	1466.412612	16.836032
29.167427	1463.403317	16.841050
29.807026	1466.277981	16.846067
29.385412	1484.742539	16.851085
29.669469	1489.497794	16.856103
29.493384	1485.550978	16.861120
29.634858	1486.328294	16.866138
29.710405	1487.336754	16.871155
29.712134	1480.790973	16.876173
29.620264	1483.927837	16.881191
29.689618	1491.772153	16.886208
29.325094	1483.595753	16.891226
30.027495	1483.971750	16.896243
29.741717	1488.298987	16.901261
29.734464	1493.452538	16.906279
30.203098	1482.499791	16.911296
29.894001	1483.313378	16.916314
29.864443	1473.866615	16.921331
29.838251	1503.576338	16.926349
30.099367	1514.436459	16.931367
30.432796	1517.938630	16.936384
30.293232	1529.021255	16.941402
30.474101	1507.681409	16.946419
29.905459	1500.243570	16.951437
30.034619	1499.620131	16.956455
30.209207	1517.090050	16.961472
30.075104	1520.216775	16.966490
30.400547	1514.167621	16.971507
30.389675	1516.526234	16.976525
30.564900	1508.196462	16.981543
30.529561	1505.914967	16.986560
30.617068	1511.727591	16.991578
30.609508	1509.067926	16.996595
30.470010	1514.318132	17.001613
30.480840	1509.267318	17.006631
30.614323	1503.049912	17.011648
30.227033	1511.534003	17.016666
30.134731	1510.548387	17.021683
30.523962	1514.514902	17.026701
30.521421	1514.120289	17.031719
30.484365	1515.396149	17.036736
30.214706	1523.000670	17.041754
30.985752	1535.908384	17.046771
30.919705	1544.812386	17.051789
30.615111	1543.577629	17.056807
31.194064	1540.917877	17.061824
30.758220	1549.098630	17.066842
30.834021	1544.947398	17.071859
30.977052	1539.227556	17.076877
31.042514	1548.512932	17.081895
31.333408	1537.819216	17.086912
30.824736	1541.083425	17.091930
31.243849	1539.577716	17.096947
31.359123	1545.348366	17.101965
31.352315	1544.415148	17.106983
31.533041	1535.074724	17.112000
31.290326	1537.513379	17.117018
31.624691	1536.416512	17.122035
31.432764	1533.225562	17.127053
31.228604	1529.464849	17.132071
31.525306	1527.484741	17.137088
31.638036	1543.159606	17.142106
31.472318	1525.729132	17.147123
31.380232	1527.281969	17.152141
31.306866	1531.035201	17.157159
31.569915	1526.553459	17.162176
31.424918	1530.264992	17.167194
31.513151	1537.843840	17.172211
31.229814	1534.965599	17.177229
31.404043	1538.972374	17.182247
31.657102	1539.436601	17.187264
31.455449	1547.161574	17.192282
31.754835	1533.472504	17.197299
31.901869	1543.660042	17.202317
31.898351	1544.109588	17.207335
31.998340	1535.149984	17.212352
31.914067	1542.693962	17.217370
31.825401	1539.062570	17.222387
31.768596	1539.694131	17.227405
31.503125	1539.358318	17.232423
31.920553	1549.004974	17.237440
32.091586	1536.202368	17.242458
31.940053	1532.940184	17.247475
31.816477	1539.856082	17.252493
31.694334	1561.158122	17.257511
31.903057	1559.386817	17.262528
31.923402	1566.665515	17.267546
31.953259	1567.809076	17.272563
31.696209	1572.862609	17.277581
31.801341	1587.313517	17.282599
31.940897	1581.449171	17.287616
31.915232	1588.707927	17.292634
32.205957	1589.417872	17.297651
32.410788	1590.361082	17.302669
32.413615	1596.480416	17.307687
32.826706	1580.860126	17.312704
32.970736	1593.690617	17.317722
33.242281	1579.523089	17.322739
32.963874	1574.265156	17.327757
32.517279	1556.699192	17.332775
32.599096	1554.258582	17.337792
32.697332	1566.105784	17.342810
32.774105	1561.756575	17.347827
32.680877	1562.807888	17.352845
32.673914	1552.238767	17.357863
32.831464	1548.721984	17.362880
32.824930	1549.920960	17.367898
32.853033	1554.678379	17.372915
33.115064	1554.288858	17.377933
32.758331	1557.220911	17.382951
32.881024	1551.116674	17.387968
32.849590	1558.200601	17.392986
32.952968	1569.262004	17.398003
33.023610	1573.247327	17.403021
32.675445	1585.485993	17.408039
32.977908	1578.602318	17.413056
32.857892	1588.083113	17.418074
32.839623	1580.952471	17.423091
32.981527	1595.091635	17.428109
32.931781	1587.574698	17.433127
33.296582	1573.164626	17.438144
33.008782	1575.452487	17.443162
33.304158	1598.091333	17.448179
33.552966	1608.185922	17.453197
33.317247	1607.025202	17.458215
33.644495	1607.802727	17.463232
33.515325	1612.685552	17.468250
33.336898	1610.686910	17.473267
33.566168	1607.082089	17.478285
33.589264	1605.734128	17.483303
33.842669	1587.212192	17.488320
33.812274	1601.000742	17.493338
33.623364	1598.011423	17.498355
33.997040	1608.046013	17.503373
33.449976	1625.527641	17.508391
33.830540	1620.667436	17.513408
33.574106	1616.822240	17.518426
33.462439	1606.966175	17.523443
33.635860	1609.651395	17.528461
33.862025	1608.204727	17.533479
33.942528	1611.259200	17.538496
33.877273	1616.414111	17.543514
34.104138	1606.901470	17.548531
34.075401	1600.665758	17.553549
34.135420	1612.149273	17.558567
34.295149	1601.831676	17.563584
34.013962	1603.331723	17.568602
33.907441	1607.328222	17.573619
34.198191	1602.273833	17.578637
33.756215	1605.086137	17.583655
34.151684	1619.673329	17.588672
34.308351	1631.826444	17.593690
34.277839	1641.971346	17.598707
34.239095	1639.753773	17.603725
34.156387	1634.416635	17.608743
34.499908	1632.510264	17.613760
34.423516	1632.887415	17.618778
34.606437	1642.515604	17.623795
34.728921	1634.818429	17.628813
34.389886	1646.911555	17.633831
34.912848	1627.534090	17.638848
34.855218	1631.005642	17.643866
34.697003	1627.992744	17.648883
35.100896	1625.681361	17.653901
35.004243	1635.741530	17.658919
34.984440	1630.934885	17.663936
34.654530	1628.882345	17.668954
35.101892	1632.030711	17.673971
35.154383	1634.226131	17.678989
34.826115	1634.142400	17.684007
34.730117	1623.469649	17.689024
34.832009	1627.867690	17.694042
34.572377	1624.408609	17.699059
35.112972	1614.614027	17.704077
35.052250	1623.726030	17.709095
35.032887	1624.302593	17.714112
35.167741	1628.749316	17.719130
35.052670	1636.784991	17.724147
35.104011	1620.660917	17.729165
35.154847	1624.409001	17.734183
34.972716	1626.428253	17.739200
35.049589	1634.027921	17.744218
34.854175	1648.851352	17.749235
35.430914	1649.886439	17.754253
35.295430	1654.143811	17.759271
35.365361	1658.570763	17.764288
35.355538	1658.383626	17.769306
35.215944	1654.541158	17.774323
35.338943	1653.387685	17.779341
35.587931	1653.024921	17.784359
35.649743	1668.479611	17.789376
35.628438	1655.759473	17.794394
35.613883	1661.150482	17.799411
36.246703	1660.323742	17.804429
36.099816	1660.204920	17.809447
35.772416	1638.426104	17.814464
36.102680	1649.606159	17.819482
35.990613	1652.134844	17.824499
35.917355	1652.219383	17.829517
35.871533	1646.079380	17.834535
35.821408	1649.004873	17.839552
36.219800	1653.121470	17.844570
36.074998	1665.446265	17.849587
36.302959	1669.242839	17.854605
35.994025	1675.524339	17.859623
36.557071	1660.694065	17.864640
36.394670	1658.609116	17.869658
36.097276	1652.500840	17.874675
36.210698	1655.032812	17.879693
36.094133	1679.023769	17.884711
36.467051	1672.064834	17.889728
36.446511	1679.519025	17.894746
36.117597	1675.635402	17.899763
36.176050	1682.805900	17.904781
35.972056	1684.198327	17.909799
36.229255	1678.083033	17.914816
36.580350	1669.165115	17.919834
36.452929	1684.448554	17.924851
36.680209	1686.731032	17.929869
36.390247	1698.654294	17.934887
36.643486	1704.906879	17.939904
36.955401	1712.369724	17.944922
36.946814	1707.443695	17.949939
36.939929	1701.212598	17.954957
37.026842	1716.528557	17.959975
36.926915	1717.856157	17.964992
37.177460	1710.043107	17.970010
37.116999	1705.067191	17.975027
37.039381	1687.238944	17.980045
36.936605	1686.196195	17.985063
36.848901	1701.164852	17.990080
36.697975	1704.618180	17.995098
36.663585	1709.176153	18.000115
36.936265	1701.894433	18.005133
36.859454	1713.412051	18.010151
36.901041	1703.153275	18.015168
36.894149	1716.992763	18.020186
36.979664	1741.113202	18.025203
37.256623	1730.215574	18.030221
37.219928	1738.583001	18.035239
37.263903	1734.895789	18.040256
37.471612	1733.716896	18.045274
37.275598	1736.070903	18.050291
37.850306	1738.284954	18.055309
38.270776	1737.614549	18.060327
37.835908	1724.864278	18.065344
37.844251	1735.999768	18.070362
37.804726	1730.188972	18.075379
38.276253	1726.348245	18.080397
38.213146	1728.564355	18.085415
38.241595	1724.520496	18.090432
38.346805	1714.979275	18.095450
37.948766	1717.116690	18.100467
37.846577	1688.436720	18.105485
37.979002	1703.891588	18.110503
37.865071	1718.475659	18.115520
38.185879	1721.063717	18.120538
38.137675	1722.033986	18.125555
38.488067	1716.416217	18.130573
38.425005	1722.065435	18.135591
38.301275	1723.476882	18.140608
38.163171	1725.332194	18.145626
38.354528	1723.139375	18.150643
38.474544	1718.868006	18.155661
38.409662	1717.086193	18.160679
38.377487	1718.287058	18.165696
38.386575	1713.646462	18.170714
38.511030	1723.983111	18.175731
38.523582	1721.099242	18.180749
38.296266	1726.301440	18.185767
38.428283	1721.040195	18.190784
38.535213	1712.714513	18.195802
38.443847	1722.721704	18.200819
38.560116	1726.356255	18.205837
38.406013	1729.208009	18.210855
38.119101	1730.137812	18.215872
38.353669	1740.165951	18.220890
38.437328	1756.591431	18.225907
38.595393	1748.163785	18.230925
38.761151	1751.005597	18.235943
38.725378	1757.977548	18.240960
38.921457	1761.366265	18.245978
38.862447	1772.976841	18.250995
39.154334	1774.172777	18.256013
39.462175	1771.256047	18.261031
39.406408	1781.774863	18.266048
39.426140	1763.236218	18.271066
39.311557	1760.019646	18.276083
39.270249	1745.764111	18.281101
39.455727	1745.476007	18.286119
39.281445	1738.462008	18.291136
39.407844	1740.758802	18.296154
39.363995	1745.955686	18.301171
39.337034	1761.864072	18.306189
39.443866	1763.877123	18.311207
39.188770	1772.003324	18.316224
39.505504	1768.349370	18.321242
39.318424	1768.944009	18.326259
39.522840	1769.893401	18.331277
39.644747	1770.717858	18.336295
39.518689	1763.872239	18.341312
39.641616	1762.514460	18.346330
39.468744	1775.972217	18.351347
39.876728	1786.583480	18.356365
40.080069	1797.121886	18.361383
39.791687	1794.861299	18.366400
40.044424	1796.471147	18.371418
39.807608	1804.917934	18.376435
39.813800	1801.481218	18.381453
39.878603	1796.805408	18.386471
39.924100	1797.180334	18.391488
40.307179	1786.302331	18.396506
39.771771	1792.143397	18.401523
39.989948	1796.441964	18.406541
40.244028	1822.762807	18.411559
40.119523	1820.569221	18.416576
40.304759	1826.698460	18.421594
40.261523	1815.683227	18.426611
40.566475	1813.963113	18.431629
40.703128	1814.098784	18.436647
40.889027	1820.179687	18.441664
40.980009	1821.054332	18.446682
40.531650	1829.053064	18.451699
40.756213	1814.125639	18.456717
41.201317	1808.938009	18.461735
40.742479	1818.485367	18.466752
40.642865	1815.832200	18.471770
40.448395	1822.528465	18.476787
40.504881	1811.348739	18.481805
40.927990	1812.420248	18.486823
40.485704	1810.581707	18.491840
40.608652	1821.293437	18.496858
40.780901	1835.318172	18.501875
41.080457	1836.043795	18.506893
41.197668	1838.253744	18.511911
41.374536	1846.555824	18.516928
41.477120	1847.046108	18.521946
41.457273	1847.718026	18.526963
41.393527	1841.029778	18.531981
41.579148	1844.348594	18.536999
41.601790	1836.685138	18.542016
41.561252	1820.943129	18.547034
41.515382	1820.286008	18.552051
41.347437	1819.588042	18.557069
41.608425	1835.764640	18.562087
41.550666	1835.607271	18.567104
41.765298	1834.455177	18.572122
41.933526	1840.565187	18.577139
42.164589	1831.075335	18.582157
42.055381	1807.931018	18.587175
41.854180	1807.310785	18.592192
42.043042	1790.434941	18.597210
42.057423	1795.925931	18.602227
42.284402	1794.853287	18.607245
42.215578	1794.903633	18.612263
41.954891	1799.393525	18.617280
42.495211	1801.831751	18.622298
42.135187	1803.990058	18.627315
41.970838	1799.752863	18.632333
42.303752	1807.574258	18.637351
42.246807	1804.909909	18.642368
42.219899	1792.716517	18.647386
42.109150	1788.782642	18.652403
42.376615	1796.739244	18.657421
42.120911	1795.271802	18.662439
41.888441	1815.598426	18.667456
41.971943	1820.483374	18.672474
42.668165	1825.524726	18.677491
41.949390	1828.653649	18.682509
41.995675	1821.466563	18.687527
42.186403	1834.244267	18.692544
42.280008	1833.692433	18.697562
42.362365	1851.138802	18.702579
42.281251	1867.262723	18.707597
42.692528	1866.526515	18.712615
42.565814	1865.129081	18.717632
42.478570	1861.882381	18.722650
42.684526	1861.777292	18.727667
42.788867	1871.070216	18.732685
43.001551	1868.095971	18.737703
42.818611	1890.752285	18.742720
42.781216	1896.995500	18.747738
43.193780	1891.126865	18.752755
43.116410	1896.800359	18.757773
43.369128	1891.759641	18.762791
43.292961	1891.152598	18.767808
43.344326	1888.370149	18.772826
43.590597	1887.364777	18.777843
43.722838	1890.686323	18.782861
43.891795	1887.097112	18.787879
43.627857	1895.553942	18.792896
43.648780	1892.405296	18.797914
43.580927	1887.798423	18.802931
43.551577	1881.215289	18.807949
43.871114	1882.242901	18.812967
43.633721	1885.506836	18.817984
43.748097	1883.417454	18.823002
44.047654	1883.830116	18.828019
43.612230	1877.313693	18.833037
43.721090	1877.213232	18.838055
43.535859	1893.788203	18.843072
43.410073	1879.520916	18.848090
43.753349	1875.466328	18.853107
43.896327	1883.217780	18.858125
43.957156	1890.296848	18.863143
44.197675	1905.332320	18.868160
43.982469	1908.094410	18.873178
44.413831	1917.691362	18.878195
43.943070	1915.039475	18.883213
44.372743	1911.911068	18.888231
44.418582	1908.267795	18.893248
44.705452	1899.883540	18.898266
44.473716	1905.401066	18.903283
44.266504	1925.028249	18.908301
44.376355	1904.958928	18.913319
44.421575	1906.073009	18.918336
44.739301	1894.563268	18.923354
44.929914	1891.597783	18.928371
44.858744	1911.121964	18.933389
45.160743	1902.424212	18.938407
44.495336	1906.512355	18.943424
44.870567	1906.584786	18.948442
44.961505	1910.713877	18.953459
44.861119	1907.316203	18.958477
44.720180	1904.861762	18.963495
44.496526	1900.363301	18.968512
44.645561	1913.267634	18.973530
44.856149	1920.476483	18.978547
45.142293	1921.473398	18.983565
45.502996	1919.678711	18.988583
45.618016	1906.106778	18.993600
45.369346	1911.168878	18.998618
45.797333	1911.873873	19.003635
45.441291	1923.591318	19.008653
45.679185	1906.623788	19.013671
45.650532	1883.700080	19.018688
45.562786	1871.976479	19.023706
45.515803	1869.819284	19.028723
45.167899	1883.855614	19.033741
45.558883	1902.732011	19.038759
45.594891	1910.162994	19.043776
45.686532	1903.992496	19.048794
45.988691	1903.333564	19.053811
46.161814	1913.495975	19.058829
45.986694	1907.422898	19.063847
46.220201	1905.383113	19.068864
46.166331	1907.292830	19.073882
46.112416	1909.588542	19.078899
45.939588	1919.147750	19.083917
46.528770	1906.800693	19.088935
45.962964	1910.586184	19.093952
46.087572	1904.140774	19.098970
46.118649	1913.312378	19.103987
45.764511	1918.639524	19.109005
46.249243	1907.244487	19.114023
46.296010	1901.240446	19.119040
45.761877	1897.797531	19.124058
46.289408	1904.346180	19.129075
46.166122	1939.146938	19.134093
46.415551	1928.905632	19.139111
46.410050	1936.817067	19.144128
46.519463	1936.518303	19.149146
46.509410	1932.858277	19.154163
46.103456	1939.634812	19.159181
46.462475	1942.623448	19.164199
46.495109	1958.669223	19.169216
46.956013	1964.273478	19.174234
46.935701	1962.146112	19.179251
46.875019	1960.046675	19.184269
46.987057	1966.597676	19.189287
47.010916	1966.643730	19.194304
47.267842	1967.335660	19.199322
47.393829	1963.897220	19.204339
47.260546	1969.263866	19.209357
47.093682	1953.544958	19.214375
47.230609	1965.692151	19.219392
46.961328	1977.779322	19.224410
47.232900	1972.837422	19.229427
47.266474	1986.186057	19.234445
47.557844	1987.869062	19.239463
47.550962	2002.011731	19.244480
47.610423	1996.835605	19.249498
47.832530	1998.380463	19.254515
47.679258	1996.139248	19.259533
47.844358	1991.712926	19.264551
47.859052	1998.001899	19.269568
47.618222	1995.638747	19.274586
47.824958	2001.684392	19.279603
47.775932	1997.527290	19.284621
47.693038	1992.462673	19.289639
48.049866	1995.273153	19.294656
48.078663	1989.111825	19.299674
48.799041	1988.796149	19.304691
48.218535	2007.837146	19.309709
48.386904	1986.994332	19.314727
48.418338	1987.346194	19.319744
48.299187	1980.852851	19.324762
48.452338	1990.073417	19.329779
48.656757	1995.173458	19.334797
48.585699	1993.190879	19.339815
48.661319	1988.687619	19.344832
48.569167	1990.643826	19.349850
48.755613	1989.858946	19.354867
48.588033	1993.055663	19.359885
48.753038	1992.276491	19.364903
48.509460	1989.615984	19.369920
48.323450	1989.849067	19.374938
48.598859	1988.969572	19.379955
48.212351	1998.436589	19.384973
48.573938	2010.597476	19.389991
48.555251	2018.425115	19.395008
48.480606	2026.972183	19.400026
48.787666	2015.712521	19.405043
48.974806	2023.428401	19.410061
49.162590	2032.399982	19.415079
48.972803	2047.588976	19.420096
49.072408	2047.823481	19.425114
49.050138	2041.338707	19.430131
49.126694	2044.334476	19.435149
49.613724	2043.801474	19.440167
49.540204	2037.268679	19.445184
49.738845	2045.393266	19.450202
49.975713	2033.174992	19.455219
49.758283	2045.983314	19.460237
49.820318	2046.142144	19.465255
49.788018	2036.066800	19.470272
49.815179	2035.886342	19.475290
49.909660	2029.237410	19.480307
50.088125	2038.637272	19.485325
49.819137	2045.496525	19.490343
49.581058	2031.954880	19.495360
49.530426	2036.597909	19.500378
49.717707	2040.919169	19.505395
49.672619	2055.312275	19.510413
49.986431	2044.970693	19.515431
50.188654	2060.088229	19.520448
49.741765	2062.957129	19.525466
49.910355	2061.843136	19.530483
50.221398	2075.758351	19.535501
50.550284	2081.745460	19.540519
50.491392	2081.390260	19.545536
50.561340	2096.628697	19.550554
50.671906	2089.172420	19.555571
50.467156	2095.824246	19.560589
50.934097	2091.025798	19.565607
51.067030	2086.619723	19.570624
50.595458	2088.989793	19.575642
50.679299	2086.681038	19.580659
50.807515	2089.422825	19.585677
50.975062	2081.611297	19.590695
50.921486	2072.881465	19.595712
50.811425	2086.049017	19.600730
51.011769	2078.858793	19.605747
50.649415	2088.021700	19.610765
50.840061	2082.149904	19.615783
51.542128	2101.954591	19.620800
51.330240	2108.593035	19.625818
51.363590	2114.001679	19.630835
51.470017	2118.551659	19.635853
51.324693	2119.548040	19.640871
51.430417	2114.652594	19.645888
51.648562	2119.979328	19.650906
51.645236	2104.533417	19.655923
51.569501	2120.142775	19.660941
51.932892	2119.709527	19.665959
52.004778	2114.178775	19.670976
51.939779	2116.707829	19.675994
51.854287	2119.077289	19.681011
51.847608	2109.986762	19.686029
51.835941	2125.329455	19.691047
51.980378	2112.410305	19.696064
51.810575	2111.965369	19.701082
51.895133	2107.933395	19.706099
51.812948	2111.025678	19.711117
52.017651	2114.746881	19.716135
52.184828	2114.184454	19.721152
51.708029	2114.598847	19.726170
51.956392	2116.491715	19.731187
52.165864	2129.546073	19.736205
52.219706	2127.791048	19.741223
52.519709	2134.875585	19.746240
52.472306	2141.949427	19.751258
52.913337	2135.337075	19.756275
52.752034	2134.111658	19.761293
52.553473	2136.794862	19.766311
52.960418	2129.604133	19.771328
52.926261	2142.403311	19.776346
52.842279	2128.473545	19.781363
52.715788	2137.554202	19.786381
52.783521	2141.820251	19.791399
52.935422	2147.845883	19.796416
53.192355	2154.589343	19.801434
52.981327	2155.144846	19.806451
53.267549	2159.547617	19.811469
53.137825	2163.335510	19.816487
53.577826	2158.287182	19.821504
53.311743	2159.780454	19.826522
53.413193	2157.223521	19.831539
53.782870	2150.456431	19.836557
53.422446	2165.603271	19.841575
53.761336	2153.895564	19.846592
53.800408	2160.507717	19.851610
53.911770	2151.531507	19.856627
54.141261	2153.045439	19.861645
53.847562	2156.893693	19.866663
54.209289	2149.118148	19.871680
53.812640	2159.919321	19.876698
54.177657	2147.794733	19.881715
53.953053	2149.811033	19.886733
53.616060	2141.556704	19.891751
53.992433	2141.203981	19.896768
54.100101	2150.242606	19.901786
53.674011	2142.919271	19.906803
54.397037	2145.633836	19.911821
54.432631	2154.969195	19.916839
54.597161	2161.287606	19.921856
54.200274	2162.258242	19.926874
54.555476	2166.915542	19.931891
54.077285	2159.875394	19.936909
54.210057	2165.907344	19.941927
54.705021	2172.164071	19.946944
54.792259	2184.772960	19.951962
54.497031	2168.007602	19.956979
54.988220	2159.285136	19.961997
54.673332	2164.984198	19.967015
54.970013	2158.319908	19.972032
54.837891	2167.650511	19.977050
54.762221	2164.372900	19.982067
54.591082	2171.041446	19.987085
54.684803	2200.896267	19.992103
55.012233	2197.001684	19.997120
55.103362	2196.391195	20.002138
55.330378	2190.512758	20.007155
55.330315	2191.775474	20.012173
55.169650	2192.447056	20.017191
55.150224	2185.791095	20.022208
55.105456	2202.882321	20.027226
55.338727	2207.907592	20.032243
55.506253	2217.011753	20.037261
55.649073	2221.515202	20.042279
55.938564	2217.785927	20.047296
55.496355	2225.005553	20.052314
55.653344	2213.772711	20.057331
56.112098	2208.024662	20.062349
56.060447	2220.896672	20.067367
56.073279	2215.042399	20.072384
55.993222	2221.277047	20.077402
55.935460	2218.250385	20.082419
55.946470	2224.391645	20.087437
55.705985	2235.500113	20.092455
55.905470	2236.307053	20.097472
56.159108	2251.552885	20.102490
55.980750	2248.459537	20.107507
56.500933	2238.485666	20.112525
56.471267	2256.897792	20.117543
56.578361	2251.843425	20.122560
56.532618	2269.455914	20.127578
56.646565	2253.380870	20.132595
57.243936	2257.660998	20.137613
56.928670	2265.198817	20.142631
57.576895	2260.896311	20.147648
57.500842	2252.462986	20.152666
57.441829	2244.007757	20.157683
57.509653	2221.706538	20.162701
57.007070	2219.765514	20.167719
57.262008	2221.263241	20.172736
57.364944	2229.196078	20.177754
57.563173	2229.043645	20.182771
57.814883	2219.509595	20.187789
57.582194	2220.712729	20.192807
57.459829	2215.256557	20.197824
57.457093	2228.531683	20.202842
57.614523	2229.689643	20.207859
57.489530	2219.300188	20.212877
57.179505	2222.717917	20.217895
57.566741	2212.286341	20.222912
57.487221	2229.169968	20.227930
57.559781	2249.053870	20.232947
57.563563	2252.772090	20.237965
57.558980	2248.783942	20.242983
57.821502	2248.663008	20.248000
57.897906	2258.582000	20.253018
57.992153	2257.708413	20.258035
58.355001	2265.760514	20.263053
58.109136	2285.970094	20.268071
58.595995	2289.238049	20.273088
58.518808	2290.166689	20.278106
58.450819	2284.482033	20.283123
58.842470	2282.970756	20.288141
58.366860	2284.421109	20.293159
58.664776	2286.722318	20.298176
58.710358	2293.663746	20.303194
58.747862	2285.457489	20.308211
58.781463	2277.752045	20.313229
58.671615	2281.353230	20.318247
58.744577	2280.247348	20.323264
59.183644	2279.820684	20.328282
58.771839	2275.353399	20.333299
58.979926	2277.780861	20.338317
58.936721	2269.256081	20.343335
58.986655	2272.470649	20.348352
59.006187	2279.393148	20.353370
58.648843	2281.258969	20.358387
59.262742	2290.441962	20.363405
58.929857	2303.334137	20.368423
59.242961	2293.771001	20.373440
59.686900	2308.255176	20.378458
59.404137	2301.888333	20.383475
59.603850	2297.897908	20.388493
59.619423	2304.450624	20.393511
59.876587	2298.759081	20.398528
60.010110	2301.431136	20.403546
59.876497	2305.690937	20.408563
59.816306	2299.018436	20.413581
59.870742	2308.149606	20.418599
59.822627	2323.624889	20.423616
60.110920	2332.548543	20.428634
59.997787	2337.942299	20.433651
60.309392	2330.016295	20.438669
60.356696	2325.114886	20.443687
60.473705	2325.740589	20.448704
60.530470	2331.979837	20.453722
60.171009	2332.270520	20.458739
60.451540	2337.990147	20.463757
60.366786	2328.408880	20.468775
59.976700	2327.015359	20.473792
60.394130	2345.362765	20.478810
60.606628	2350.664531	20.483827
60.420637	2358.492234	20.488845
60.262241	2368.136138	20.493863
60.835482	2377.787489	20.498880
61.135108	2387.058100	20.503898
61.272478	2373.075789	20.508915
61.611852	2380.084056	20.513933
61.660725	2378.537291	20.518951
61.837327	2366.894034	20.523968
61.730442	2345.303749	20.528986
61.424059	2349.242920	20.534003
61.868130	2337.741696	20.539021
61.700229	2334.397798	20.544039
61.988262	2318.562800	20.549056
62.047711	2326.150730	20.554074
61.571010	2344.207329	20.559091
61.802773	2339.429362	20.564109
61.541452	2341.012803	20.569127
61.510446	2336.615245	20.574144
61.864987	2341.661267	20.579162
61.812194	2355.944122	20.584179
61.984563	2359.312481	20.589197
61.834685	2366.876757	20.594215
61.877267	2365.627078	20.599232
62.239252	2367.356329	20.604250
62.315133	2372.659025	20.609267
62.200655	2363.845594	20.614285
62.409698	2369.926237	20.619303
62.770616	2384.740326	20.624320
62.540612	2389.506994	20.629338
62.822264	2402.449663	20.634355
63.211848	2397.397581	20.639373
62.978285	2381.442029	20.644391
62.518140	2378.868418	20.649408
62.668117	2377.632092	20.654426
62.727669	2374.554520	20.659443
62.916720	2380.675083	20.664461
62.796468	2390.163888	20.669479
63.352479	2387.080650	20.674496
63.178766	2390.631394	20.679514
62.641948	2394.676760	20.684531
62.726790	2385.127272	20.689549
62.887350	2399.703239	20.694567
63.119593	2419.040728	20.699584
63.356057	2413.193123	20.704602
63.186137	2431.696346	20.709619
63.633164	2416.360144	20.714637
63.579137	2430.281087	20.719655
63.862315	2421.807009	20.724672
63.822887	2420.295696	20.729690
63.691850	2428.609208	20.734707
64.195969	2436.005609	20.739725
63.908995	2445.560578	20.744743
64.235751	2438.892576	20.749760
64.530221	2442.292350	20.754778
64.067483	2446.506186	20.759795
64.571326	2444.448825	20.764813
65.014775	2439.953546	20.769831
64.822638	2427.148408	20.774848
65.037956	2403.026986	20.779866
64.753651	2399.620818	20.784883
65.174721	2393.045119	20.789901
65.066104	2391.909394	20.794919
64.653534	2396.541280	20.799936
64.859998	2397.299834	20.804954
64.788219	2402.131694	20.809971
64.648858	2389.298576	20.814989
64.982385	2392.117902	20.820007
64.953449	2396.684033	20.825024
64.958232	2397.294035	20.830042
64.866300	2414.826532	20.835059
64.718216	2434.955586	20.840077
64.805103	2421.671692	20.845095
64.686949	2426.068727	20.850112
64.871218	2434.978529	20.855130
65.130930	2456.330706	20.860147
65.194435	2481.021852	20.865165
65.428929	2472.112901	20.870183
65.331757	2473.062571	20.875200
65.649806	2480.547217	20.880218
65.649259	2483.181225	20.885235
66.068728	2477.443113	20.890253
66.243877	2482.657007	20.895271
66.107908	2486.658598	20.900288
66.409075	2466.539613	20.905306
66.751892	2473.760335	20.910323
66.435175	2473.916405	20.915341
66.511912	2481.426361	20.920359
66.361328	2477.953199	20.925376
66.434903	2473.056849	20.930394
66.717560	2471.431289	20.935411
66.654081	2473.558399	20.940429
66.695072	2480.134547	20.945447
66.812397	2473.281464	20.950464
67.080742	2469.136749	20.955482
66.883289	2475.848354	20.960499
66.927297	2476.897916	20.965517
66.869522	2474.841234	20.970535
66.837683	2478.072900	20.975552
66.869595	2464.965761	20.980570
66.916218	2473.200336	20.985587
66.683454	2470.038771	20.990605
66.974848	2487.658001	20.995623
66.901506	2498.360318	21.000640
66.879975	2503.170520	21.005658
67.160126	2498.971880	21.010675
67.416371	2493.099325	21.015693
67.254652	2504.902414	21.020711
67.206777	2528.927825	21.025728
67.537678	2531.594075	21.030746
67.582424	2533.119087	21.035763
67.854036	2522.751682	21.040781
67.836714	2519.274599	21.045799
67.667758	2532.807560	21.050816
67.921649	2545.788399	21.055834
67.991024	2561.270095	21.060851
68.400524	2564.594985	21.065869
68.462693	2567.427296	21.070887
68.414676	2553.768749	21.075904
68.263947	2560.067177	21.080922
68.634615	2547.707103	21.085939
68.310449	2554.685732	21.090957
68.842503	2554.170866	21.095975
68.817087	2549.580994	21.100992
69.062383	2538.325057	21.106010
69.053860	2549.222987	21.111027
69.220760	2536.049389	21.116045
69.282223	2538.360183	21.121063
68.990364	2536.832306	21.126080
69.524281	2535.409303	21.131098
69.240163	2548.585735	21.136115
69.097406	2539.619010	21.141133
69.367584	2534.613780	21.146151
69.282083	2535.073359	21.151168
69.523525	2531.251167	21.156186
69.486103	2526.062922	21.161203
69.605186	2534.065094	21.166221
69.854303	2540.588768	21.171239
69.287576	2547.561808	21.176256
69.479426	2551.362403	21.181274
69.767628	2558.858713	21.186291
69.665938	2565.375013	21.191309
69.918709	2564.134679	21.196327
69.714470	2561.378205	21.201344
70.138479	2576.483221	21.206362
70.192618	2587.025563	21.211379
69.903582	2588.861629	21.216397
70.393064	2592.984690	21.221415
70.602119	2588.234807	21.226432
70.588800	2584.742875	21.231450
70.731403	2591.505815	21.236467
70.596200	2591.474025	21.241485
70.732914	2591.234711	21.246503
70.506226	2590.961357	21.251520
70.493500	2576.379677	21.256538
70.440474	2606.934501	21.261555
70.599204	2616.013187	21.266573
71.051640	2611.299849	21.271591
70.476608	2620.660016	21.276608
71.057070	2624.837734	21.281626
71.417125	2647.037729	21.286643
71.820406	2638.779110	21.291661
71.561543	2638.525244	21.296679
71.600019	2655.602625	21.301696
71.924713	2651.762316	21.306714
71.783389	2640.621764	21.311731
71.834638	2648.854881	21.316749
72.193695	2643.906973	21.321767
71.933870	2647.658611	21.326784
71.896477	2645.609561	21.331802
72.158849	2638.425364	21.336819
71.940502	2646.212103	21.341837
72.125635	2647.774162	21.346855
71.896479	2645.185956	21.351872
71.952145	2637.490663	21.356890
72.450598	2636.947491	21.361907
72.287368	2635.747153	21.366925
72.606418	2640.142867	21.371943
72.216290	2651.190536	21.376960
72.119425	2645.935698	21.381978
72.241404	2658.470733	21.386995
72.685697	2662.280033	21.392013
72.720592	2662.489809	21.397031
72.666509	2667.893607	21.402048
72.832956	2669.104439	21.407066
72.886262	2671.675252	21.412083
72.737942	2690.876761	21.417101
72.894076	2688.924068	21.422119
72.776853	2703.369065	21.427136
72.955699	2697.260020	21.432154
73.287795	2698.769847	21.437171
73.103017	2720.024583	21.442189
74.066728	2714.572424	21.447207
73.987132	2715.955013	21.452224
73.805784	2724.051021	21.457242
74.023026	2719.642647	21.462259
74.443696	2716.574623	21.467277
74.529583	2709.272711	21.472295
74.650416	2703.481112	21.477312
74.476812	2693.471797	21.482330
74.372085	2688.025337	21.487347
74.382210	2687.866387	21.492365
74.500842	2682.863711	21.497383
74.376416	2677.644912	21.502400
74.262654	2679.199279	21.507418
74.322694	2690.994211	21.512435
74.238775	2710.391001	21.517453
75.067555	2703.650167	21.522471
74.895847	2711.786699	21.527488
74.600859	2700.973059	21.532506
74.489704	2708.450790	21.537523
74.126073	2727.117471	21.542541
74.609275	2728.989721	21.547559
75.008993	2738.879808	21.552576
74.579545	2732.422068	21.557594
75.251299	2743.209693	21.562611
75.416458	2768.351414	21.567629
75.930101	2758.186371	21.572647
75.606569	2765.775991	21.577664
75.829062	2756.916890	21.582682
75.979106	2755.278964	21.587699
75.468575	2766.888718	21.592717
76.195691	2753.675513	21.597735
76.171506	2760.277116	21.602752
75.960820	2754.536342	21.607770
76.204232	2751.247611	21.612787
75.813574	2768.499961	21.617805
76.216588	2754.290346	21.622823
76.428912	2756.383337	21.627840
76.315754	2754.473165	21.632858
76.563078	2758.633136	21.637875
76.352158	2756.113943	21.642893
76.703950	2759.002365	21.647911
76.727736	2766.808995	21.652928
76.965672	2774.684570	21.657946
76.801145	2784.041173	21.662963
76.802294	2792.068084	21.667981
76.835853	2786.659368	21.672999
76.734706	2795.851179	21.678016
76.474282	2782.027142	21.683034
76.534418	2781.256403	21.688051
77.022672	2802.238233	21.693069
77.478329	2807.003930	21.698087
77.652181	2816.749506	21.703104
77.552126	2818.870896	21.708122
77.816975	2804.125029	21.713139
77.540480	2805.094113	21.718157
77.728519	2800.032688	21.723175
77.663872	2801.056528	21.728192
77.688699	2810.470831	21.733210
78.078532	2804.774504	21.738227
77.934976	2814.841023	21.743245
78.083026	2810.175167	21.748263
78.164463	2816.624307	21.753280
78.049606	2837.669625	21.758298
78.115015	2842.924214	21.763315
78.060361	2841.227980	21.768333
78.693296	2836.964656	21.773351
78.556086	2831.045181	21.778368
78.618928	2835.094323	21.783386
78.774927	2840.041825	21.788403
78.536148	2840.554693	21.793421
79.115919	2847.094723	21.798439
79.299666	2857.775671	21.803456
79.233692	2867.816807	21.808474
79.220486	2869.565989	21.813491
79.407828	2865.245189	21.818509
79.383325	2863.727036	21.823527
79.261122	2866.919780	21.828544
79.334293	2864.235518	21.833562
79.516580	2854.834201	21.838579
79.154305	2859.010288	21.843597
79.328775	2861.452059	21.848615
79.405146	2873.985750	21.853632
79.516771	2893.298882	21.858650
79.925562	2890.733169	21.863667
79.537484	2898.331552	21.868685
79.879589	2887.561321	21.873703
79.676364	2900.130998	21.878720
79.580955	2917.824083	21.883738
80.271118	2915.400450	21.888755
79.901331	2914.073989	21.893773
80.352016	2923.837274	21.898791
80.602671	2939.520490	21.903808
80.879106	2936.847509	21.908826
81.417558	2916.507634	21.913843
81.713779	2919.845809	21.918861
81.662175	2904.290347	21.923879
81.369206	2894.539990	21.928896
81.397522	2899.305859	21.933914
81.439835	2881.907781	21.938931
81.601527	2886.833886	21.943949
81.632672	2889.861535	21.948967
81.633770	2885.863623	21.953984
81.348360	2892.368294	21.959002
81.935705	2878.847379	21.964019
81.625085	2877.367448	21.969037
81.603438	2883.943095	21.974055
81.926539	2878.406189	21.979072
81.659743	2888.238403	21.984090
81.901930	2889.363905	21.989107
81.953044	2910.229538	21.994125
82.397014	2895.138639	21.999143
82.482183	2914.090432	22.004160
82.188029	2903.265881	22.009178
82.583051	2907.878247	22.014195
82.557304	2911.747564	22.019213
82.197838	2908.472596	22.024231
82.467727	2903.936181	22.029248
82.310837	2915.728155	22.034266
82.378087	2911.825602	22.039283
82.838504	2927.873349	22.044301
82.819815	2935.700075	22.049319
82.717349	2939.877344	22.054336
82.834002	2933.741476	22.059354
83.094715	2934.828094	22.064371
82.973261	2939.428964	22.069389
83.017658	2937.665566	22.074407
83.193775	2955.136272	22.079424
83.105995	2963.497645	22.084442
83.197728	2957.535567	22.089459
83.413130	2976.316706	22.094477
83.686653	2980.610201	22.099495
83.511633	2991.523356	22.104512
83.545873	3009.291577	22.109530
84.028532	3001.198781	22.114547
84.078900	2998.988728	22.119565
83.750404	3006.113152	22.124583
84.272535	3002.234623	22.129600
84.678903	3025.970789	22.134618
84.622904	3025.672370	22.139635
84.457404	3024.708199	22.144653
84.946974	3023.347994	22.149671
84.829007	3029.670726	22.154688
84.325595	3030.135990	22.159706
84.841083	3021.991697	22.164723
85.247051	3023.404313	22.169741
84.979534	3014.893353	22.174759
84.791684	3016.578104	22.179776
84.967158	3016.233957	22.184794
85.100910	3022.093839	22.189811
85.378758	3037.673451	22.194829
85.330394	3046.827556	22.199847
85.821984	3041.137163	22.204864
85.559720	3034.856784	22.209882
85.519329	3049.129961	22.214899
85.587432	3049.988576	22.219917
85.595475	3040.243898	22.224935
85.800424	3056.076516	22.229952
85.366276	3071.349803	22.234970
85.717161	3068.953076	22.239987
86.203999	3076.833346	22.245005
86.039543	3111.550433	22.250023
86.699835	3094.866134	22.255040
86.529052	3093.302052	22.260058
86.902510	3091.425601	22.265075
86.982872	3103.970236	22.270093
86.858327	3095.094273	22.275111
87.025256	3096.871982	22.280128
87.215793	3094.092697	22.285146
87.130299	3085.928387	22.290163
86.956085	3080.008239	22.295181
86.751971	3085.312171	22.300199
87.165698	3090.264804	22.305216
87.198120	3088.491557	22.310234
87.596059	3102.396687	22.315251
87.462628	3112.718023	22.320269
87.289137	3116.212990	22.325287
88.001785	3117.991077	22.330304
87.923361	3111.536196	22.335322
87.809148	3114.078465	22.340339
87.655301	3120.614640	22.345357
87.965431	3131.881580	22.350375
88.126004	3128.957243	22.355392
88.372294	3149.361817	22.360410
88.778289	3138.644242	22.365427
88.625338	3137.133901	22.370445
88.351509	3126.391267	22.375463
88.696081	3132.615170	22.380480
88.549903	3139.315439	22.385498
88.558510	3144.324401	22.390515
88.918911	3135.483242	22.395533
88.871604	3136.344791	22.400551
88.832271	3133.407422	22.405568
88.326112	3140.564021	22.410586
88.884897	3153.154049	22.415603
89.039177	3164.542828	22.420621
88.934288	3170.156769	22.425639
89.124279	3167.571655	22.430656
89.398871	3176.311844	22.435674
89.734975	3188.041459	22.440691
89.760721	3190.333449	22.445709
89.663434	3188.887133	22.450727
89.984818	3187.566910	22.455744
89.821189	3196.501175	22.460762
90.070883	3191.685733	22.465779
90.252141	3187.364669	22.470797
90.192231	3180.566151	22.475815
90.626300	3192.932727	22.480832
90.672635	3201.613798	22.485850
90.727018	3207.337260	22.490867
91.059464	3209.962824	22.495885
90.913763	3197.783229	22.500903
91.264821	3185.268804	22.505920
90.981416	3189.346906	22.510938
91.044887	3199.775526	22.515955
91.328507	3209.812660	22.520973
91.158065	3217.281140	22.525991
91.468225	3207.171871	22.531008
91.420217	3211.642575	22.536026
91.335013	3206.857664	22.541043
91.488853	3203.947417	22.546061
91.544473	3209.709258	22.551079
91.901019	3204.807259	22.556096
91.467910	3209.244353	22.561114
91.652507	3217.066370	22.566131
91.472198	3212.729847	22.571149
91.590096	3239.114387	22.576167
91.931750	3236.072313	22.581184
92.075401	3254.652655	22.586202
92.127278	3254.300973	22.591219
92.552570	3258.313563	22.596237
92.351744	3247.157209	22.601255
92.263957	3259.664007	22.606272
92.513047	3276.791522	22.611290
92.606501	3282.562099	22.616307
92.861840	3279.074437	22.621325
92.884175	3288.128419	22.626343
92.999067	3276.387197	22.631360
92.880207	3294.247972	22.636378
93.185186	3312.377315	22.641395
93.652784	3309.309692	22.646413
93.777909	3315.828986	22.651431
93.966492	3307.741318	22.656448
93.871265	3310.176938	22.661466
94.356465	3304.013097	22.666483
94.757969	3290.883559	22.671501
94.205079	3303.520395	22.676519
94.684353	3284.358324	22.681536
94.493626	3264.586908	22.686554
94.595565	3258.458068	22.691571
94.638086	3251.579995	22.696589
94.457016	3255.716795	22.701607
94.534174	3244.773169	22.706624
94.443780	3245.937118	22.711642
94.543778	3260.906581	22.716659
94.963766	3271.372796	22.721677
94.772237	3292.629824	22.726695
94.845656	3276.202936	22.731712
94.729858	3292.924622	22.736730
94.656730	3289.589659	22.741747
94.906179	3300.445490	22.746765
94.964510	3316.433703	22.751783
95.354245	3309.672641	22.756800
95.528252	3327.175218	22.761818
95.246858	3332.018774	22.766835
95.584911	3324.887898	22.771853
95.091095	3352.172137	22.776871
95.359695	3348.982663	22.781888
95.779481	3349.566254	22.786906
96.097034	3363.622699	22.791923
96.257090	3382.834738	22.796941
96.324797	3389.715128	22.801959
96.490109	3379.941494	22.806976
96.507444	3378.097477	22.811994
96.507417	3377.714606	22.817011
96.540277	3376.555429	22.822029
96.518133	3382.607351	22.827047
96.768548	3396.145783	22.832064
97.008316	3400.652455	22.837082
97.097312	3408.722651	22.842099
96.985707	3403.163295	22.847117
97.242266	3414.081417	22.852135
97.377034	3402.808080	22.857152
97.619254	3408.378924	22.862170
97.100938	3420.856597	22.867187
97.518121	3426.344599	22.872205
97.772709	3427.509038	22.877223
97.693652	3423.599036	22.882240
97.639576	3433.439751	22.887258
97.877672	3452.266143	22.892275
98.396832	3456.778634	22.897293
98.152868	3469.882280	22.902311
98.356369	3457.672338	22.907328
98.644944	3457.034687	22.912346
98.402090	3464.633363	22.917363
98.760044	3467.813819	22.922381
98.538101	3464.432934	22.927399
98.639825	3466.597449	22.932416
98.935741	3480.002056	22.937434
99.165085	3482.150210	22.942451
99.436691	3476.964914	22.947469
99.407290	3480.952694	22.952487
99.439846	3484.396767	22.957504
99.723317	3482.575692	22.962522
99.162633	3488.522939	22.967539
99.597526	3487.890244	22.972557
99.696075	3501.874340	22.977575
99.682297	3506.399710	22.982592
99.858978	3507.753803	22.987610
99.869369	3508.786155	22.992627
100.160794	3509.886639	22.997645
99.929957	3513.609283	23.002663
99.983647	3520.069206	23.007680
100.293911	3531.804533	23.012698
100.367123	3533.213915	23.017715
100.787410	3525.411082	23.022733
100.658109	3532.008335	23.027751
100.683658	3526.001069	23.032768
101.523559	3535.733894	23.037786
101.853587	3524.854589	23.042803
101.946851	3507.349752	23.047821
101.610829	3504.165271	23.052839
101.900992	3504.633277	23.057856
102.168636	3501.315976	23.062874
101.875814	3500.205094	23.067891
102.140631	3496.075258	23.072909
102.369722	3502.435324	23.077927
102.312823	3485.334857	23.082944
102.257642	3474.868848	23.087962
102.017679	3469.161778	23.092979
102.433064	3490.134144	23.097997
102.153122	3499.131109	23.103015
102.406778	3494.710594	23.108032
102.367530	3489.090826	23.113050
102.378679	3502.990545	23.118067
102.651496	3497.889295	23.123085
102.292849	3501.269270	23.128103
102.548721	3506.552064	23.133120
102.761110	3521.656359	23.138138
102.116161	3536.130274	23.143155
102.492126	3531.463552	23.148173
102.904777	3557.217243	23.153191
102.835403	3565.707397	23.158208
103.222182	3569.822498	23.163226
103.000117	3586.367566	23.168243
103.365002	3587.660252	23.173261
103.413996	3587.859444	23.178279
103.820641	3606.789672	23.183296
104.177889	3616.471984	23.188314
104.164557	3611.083721	23.193331
104.235283	3599.378294	23.198349
104.458084	3614.318358	23.203367
104.147271	3616.888469	23.208384
104.506444	3618.558881	23.213402
104.721684	3628.710344	23.218419
104.843584	3630.254212	23.223437
104.779052	3627.901635	23.228455
105.209307	3636.229347	23.233472
105.421386	3633.652319	23.238490
105.087351	3650.699826	23.243507
105.069629	3634.442742	23.248525
105.008558	3646.914727	23.253543
105.232826	3663.456207	23.258560
105.371113	3659.284242	23.263578
105.609535	3665.848350	23.268595
106.027806	3651.245232	23.273613
105.697590	3667.283048	23.278631
105.530350	3681.664776	23.283648
106.241275	3696.682534	23.288666
106.126152	3694.213500	23.293683
106.285995	3686.050068	23.298701
106.370451	3696.547604	23.303719
106.141840	3706.122835	23.308736
106.359583	3714.714844	23.313754
106.761197	3718.661781	23.318771
106.771630	3714.853851	23.323789
107.111182	3720.139820	23.328807
107.111918	3727.201903	23.333824
107.198387	3714.580377	23.338842
107.138734	3732.549197	23.343859
107.415624	3736.259654	23.348877
108.094000	3743.904675	23.353895
107.646778	3750.867948	23.358912
107.846584	3740.769481	23.363930
107.444209	3750.819921	23.368947
107.609322	3754.423258	23.373965
107.741426	3754.525646	23.378983
107.881712	3765.804184	23.384000
108.422603	3774.387320	23.389018
108.103177	3769.610227	23.394035
108.100545	3763.298462	23.399053
108.558435	3769.586972	23.404071
108.259703	3777.732057	23.409088
108.722210	3788.811695	23.414106
108.682234	3793.211159	23.419123
109.064023	3786.431126	23.424141
109.158163	3790.540309	23.429159
109.309493	3803.880501	23.434176
109.475200	3790.341855	23.439194
109.265481	3793.903197	23.444211
109.947492	3804.653260	23.449229
109.961403	3802.263678	23.454247
109.791889	3814.669461	23.459264
110.278294	3808.341834	23.464282
110.105239	3813.688520	23.469299
110.240075	3825.263681	23.474317
110.326871	3814.697996	23.479335
110.253352	3823.092909	23.484352
110.383903	3813.445224	23.489370
110.579141	3800.716283	23.494387
110.743136	3810.479075	23.499405
110.894512	3800.179511	23.504423
110.998501	3816.762683	23.509440
111.045494	3822.863590	23.514458
110.990736	3831.183751	23.519475
111.173683	3836.760607	23.524493
111.289106	3833.151843	23.529511
111.208121	3826.417943	23.534528
111.621980	3825.528468	23.539546
111.479584	3848.768363	23.544563
111.719732	3853.050687	23.549581
111.681507	3864.989132	23.554599
111.795073	3865.789098	23.559616
111.986849	3854.165450	23.564634
112.263460	3875.832553	23.569651
112.317319	3892.873712	23.574669
112.371237	3902.817356	23.579687
112.264303	3913.419500	23.584704
112.934333	3904.752739	23.589722
112.372244	3900.974795	23.594739
112.576290	3909.944387	23.599757
113.273295	3912.332270	23.604775
113.167741	3916.701263	23.609792
113.008371	3923.608781	23.614810
112.935335	3926.809758	23.619827
113.078990	3943.502264	23.624845
113.294572	3949.329290	23.629863
113.477343	3959.636341	23.634880
114.026153	3953.064476	23.639898
113.924287	3955.668229	23.644915
114.034115	3977.742576	23.649933
114.183087	3973.956181	23.654951
114.147162	3981.772501	23.659968
114.654415	3982.740109	23.664986
114.427254	3980.225760	23.670003
114.480822	3978.277256	23.675021
114.694051	3977.479588	23.680039
114.693885	4004.065258	23.685056
115.133055	3999.243459	23.690074
115.145650	4008.088043	23.695091
115.332674	4004.308740	23.700109
115.554489	3997.829078	23.705127
115.263046	3994.593031	23.710144
115.474132	3995.131997	23.715162
115.420347	4001.337819	23.720179
115.673000	4008.344229	23.725197
115.936141	4015.706013	23.730215
115.711689	4025.329573	23.735232
115.707066	4019.804290	23.740250
115.690665	4020.975362	23.745267
115.902186	4038.695781	23.750285
116.026059	4053.508513	23.755303
116.039384	4055.193992	23.760320
116.346526	4059.920445	23.765338
116.518276	4087.249149	23.770355
116.390645	4090.022938	23.775373
116.640838	4073.679786	23.780391
116.622347	4094.901441	23.785408
116.978908	4113.311008	23.790426
117.232276	4119.874021	23.795443
117.163620	4110.703187	23.800461
117.819239	4125.810427	23.805479
117.596903	4140.189869	23.810496
117.755775	4140.521708	23.815514
118.242210	4131.635933	23.820531
118.087423	4137.962441	23.825549
118.508429	4132.003778	23.830567
118.650194	4139.143143	23.835584
118.444735	4127.949910	23.840602
118.546378	4134.078132	23.845619
118.770837	4128.060209	23.850637
118.690357	4124.696358	23.855655
118.954300	4158.883945	23.860672
119.340071	4150.885314	23.865690
119.258570	4156.076430	23.870707
119.293147	4159.967193	23.875725
119.412455	4160.039807	23.880743
119.287070	4160.361920	23.885760
119.412845	4177.712786	23.890778
119.552069	4183.925768	23.895795
119.325544	4175.658196	23.900813
119.837694	4188.662312	23.905831
120.054352	4198.290261	23.910848
120.336592	4212.404496	23.915866
120.109306	4229.818483	23.920883
120.185226	4227.136683	23.925901
120.540354	4230.528014	23.930919
120.669354	4244.268362	23.935936
120.886435	4251.026414	23.940954
120.777362	4255.940605	23.945971
120.884678	4256.981009	23.950989
121.156707	4250.570116	23.956007
121.159394	4272.833854	23.961024
121.153806	4283.425409	23.966042
121.610923	4282.974854	23.971059
121.409148	4290.723844	23.976077
121.677553	4285.344705	23.981095
121.442202	4294.269399	23.986112
121.754351	4299.068331	23.991130
122.098817	4306.832984	23.996147
121.977043	4314.424664	24.001165
122.663629	4317.366732	24.006183
122.596179	4332.486163	24.011200
122.891480	4320.765137	24.016218
123.352245	4317.344885	24.021235
123.341135	4313.363978	24.026253
123.126909	4316.081638	24.031271
123.106414	4330.462158	24.036288
122.954938	4323.165244	24.041306
123.310191	4325.737230	24.046323
123.276826	4339.867113	24.051341
123.536853	4337.311577	24.056359
123.346572	4346.436742	24.061376
123.502464	4349.063328	24.066394
123.516884	4363.107772	24.071411
123.972293	4368.759886	24.076429
124.886847	4371.967468	24.081447
124.751013	4371.549134	24.086464
124.486775	4376.449235	24.091482
124.642047	4379.060574	24.096499
124.823218	4376.518061	24.101517
124.613077	4378.460200	24.106535
124.572937	4384.058366	24.111552
124.753376	4403.652184	24.116570
125.305306	4401.010607	24.121587
125.482668	4395.321647	24.126605
125.613386	4397.545286	24.131623
125.600028	4403.023277	24.136640
125.888425	4417.698926	24.141658
125.988282	4416.347487	24.146675
126.139867	4427.095466	24.151693
126.361459	4417.471738	24.156711
126.453883	4414.319035	24.161728
126.398347	4426.996650	24.166746
126.576849	4423.085574	24.171763
126.300237	4421.879811	24.176781
126.922082	4418.765229	24.181799
126.489285	4428.007683	24.186816
126.554086	4440.903631	24.191834
127.039657	4445.789711	24.196851
127.176628	4467.531502	24.201869
127.526596	4468.568837	24.206887
127.371625	4473.885986	24.211904
127.325511	4471.968459	24.216922
127.321834	4478.389437	24.221939
127.632683	4491.548338	24.226957
127.965083	4507.418074	24.231975
127.742368	4507.377900	24.236992
127.862711	4519.270563	24.242010
128.770734	4528.582496	24.247027
128.360180	4537.248853	24.252045
128.617473	4528.651918	24.257063
128.818958	4529.427943	24.262080
128.719655	4533.550386	24.267098
129.042778	4539.265370	24.272115
129.316701	4550.075509	24.277133
129.570257	4543.002142	24.282151
129.959822	4551.273681	24.287168
129.839783	4548.900605	24.292186
130.278417	4538.897606	24.297203
129.835467	4552.679970	24.302221
129.869152	4547.412365	24.307239
129.895013	4557.822911	24.312256
130.261829	4570.616304	24.317274
130.463340	4568.169227	24.322291
130.008508	4577.014983	24.327309
130.335730	4583.533309	24.332327
130.537063	4600.789872	24.337344
130.634215	4604.495589	24.342362
131.203862	4595.429254	24.347379
130.954961	4612.119618	24.352397
131.068117	4620.568766	24.357415
131.185793	4625.355048	24.362432
131.434547	4640.853275	24.367450
131.793243	4634.414913	24.372467
131.816672	4658.705083	24.377485
131.804190	4652.342612	24.382503
131.752686	4662.731362	24.387520
131.871073	4667.079706	24.392538
132.030610	4670.567238	24.397555
131.918171	4689.490847	24.402573
132.262661	4706.489992	24.407591
132.245643	4700.946436	24.412608
132.456486	4706.984392	24.417626
132.659956	4704.439718	24.422643
133.051452	4724.771577	24.427661
133.299784	4713.196220	24.432679
133.545009	4727.037092	24.437696
133.684218	4740.937228	24.442714
133.789853	4741.668466	24.447731
133.886241	4746.853221	24.452749
133.940796	4747.241685	24.457767
134.471478	4732.236668	24.462784
134.514472	4744.089129	24.467802
134.882200	4728.435388	24.472819
135.116591	4710.905883	24.477837
135.558150	4724.846214	24.482855
135.633457	4711.954442	24.487872
135.530232	4705.764044	24.492890
135.806939	4679.555931	24.497907
135.598292	4673.159323	24.502925
135.428713	4678.617156	24.507943
135.751923	4667.972458	24.512960
135.605787	4679.645472	24.517978
135.715921	4687.262012	24.522995
135.425807	4711.587929	24.528013
135.844213	4692.111724	24.533031
135.844509	4710.673787	24.538048
135.756818	4724.594470	24.543066
136.131751	4734.667116	24.548083
136.113736	4740.510595	24.553101
136.375097	4750.299626	24.558119
136.231004	4766.205048	24.563136
136.224835	4769.711714	24.568154
136.627291	4775.998378	24.573171
136.853078	4800.819167	24.578189
136.734748	4810.504815	24.583207
137.158175	4818.472054	24.588224
137.275592	4832.580224	24.593242
137.750657	4831.127774	24.598259
137.885798	4828.575864	24.603277
137.945023	4843.874878	24.608295
138.442910	4837.795756	24.613312
138.262577	4841.700544	24.618330
138.373553	4845.495775	24.623347
138.461642	4853.382207	24.628365
138.446888	4850.142391	24.633383
139.067609	4866.640512	24.638400
138.890636	4868.639441	24.643418
139.397197	4871.407408	24.648435
139.204953	4875.196444	24.653453
139.284213	4884.035627	24.658471
139.370943	4892.069168	24.663488
139.412202	4910.375462	24.668506
139.795722	4909.680728	24.673523
139.357196	4911.942193	24.678541
139.733500	4932.057913	24.683559
140.249204	4938.818109	24.688576
139.937812	4949.492537	24.693594
140.441855	4957.673323	24.698611
140.415425	4963.202100	24.703629
140.684742	4961.585582	24.708647
141.156143	4962.833227	24.713664
140.987774	4982.378308	24.718682
141.226575	4982.711923	24.723699
141.613466	4993.802556	24.728717
141.633495	4997.440787	24.733735
141.829752	4991.185829	24.738752
141.977074	4991.848767	24.743770
141.789012	4997.581841	24.748787
141.864991	4997.374974	24.753805
141.990746	5014.783868	24.758823
141.928262	5022.050310	24.763840
142.085484	5023.325855	24.768858
142.496040	5035.202853	24.773875
142.285178	5047.123476	24.778893
142.569916	5050.184062	24.783911
143.139702	5051.482395	24.788928
142.747084	5060.640226	24.793946
142.876976	5074.969020	24.798963
143.062813	5089.921727	24.803981
143.268410	5090.545902	24.808999
143.520325	5106.700052	24.814016
143.413059	5113.315592	24.819034
143.675116	5116.652805	24.824051
144.068926	5132.242921	24.829069
144.032255	5152.650810	24.834087
144.713152	5144.598187	24.839104
144.501696	5142.758297	24.844122
144.883573	5141.703152	24.849139
145.174478	5158.684477	24.854157
145.200726	5167.238450	24.859175
145.618496	5156.091125	24.864192
145.125920	5165.666368	24.869210
145.631571	5160.282774	24.874227
145.509902	5154.627592	24.879245
145.712196	5170.456896	24.884263
146.049872	5179.981983	24.889280
146.023812	5173.479006	24.894298
146.296790	5185.128034	24.899315
146.202519	5195.946696	24.904333
146.228268	5213.860584	24.909351
146.681839	5212.834539	24.914368
146.930864	5221.904162	24.919386
147.012502	5210.577664	24.924403
147.237742	5232.427209	24.929421
147.226371	5237.441720	24.934439
147.504031	5230.847586	24.939456
147.605055	5235.074926	24.944474
147.757736	5226.669326	24.949491
148.066726	5239.199168	24.954509
148.320499	5262.107953	24.959527
148.037077	5260.969003	24.964544
148.445096	5268.427932	24.969562
148.489757	5268.202217	24.974579
148.754442	5264.064855	24.979597
148.665002	5269.793152	24.984615
148.947287	5283.914651	24.989632
149.192544	5291.371346	24.994650
149.270868	5297.493247	24.999667
149.254554	5278.454334	25.004685
149.226299	5295.987425	25.009703
149.828948	5308.067568	25.014720
149.678347	5331.905192	25.019738
149.662487	5317.274607	25.024755
150.286480	5328.242434	25.029773
150.070868	5340.018376	25.034791
150.036072	5349.936256	25.039808
150.023440	5354.312739	25.044826
150.978421	5357.661120	25.049843
151.225739	5354.670457	25.054861
151.464311	5370.350249	25.059879
151.686644	5351.049345	25.064896
151.476963	5357.020799	25.069914
151.718652	5356.188831	25.074931
151.860758	5364.767869	25.079949
151.718481	5360.695361	25.084967
151.765081	5360.719752	25.089984
152.137076	5367.015234	25.095002
152.144514	5372.207807	25.100019
152.474845	5383.641180	25.105037
152.534108	5395.068161	25.110055
152.705984	5381.801960	25.115072
152.310572	5392.609878	25.120090
152.516653	5403.352281	25.125107
152.989182	5420.785049	25.130125
152.603849	5428.746844	25.135143
153.054966	5438.475817	25.140160
153.238333	5450.178043	25.145178
153.449115	5453.798642	25.150195
153.381375	5455.641388	25.155213
153.629518	5490.597600	25.160231
153.709693	5479.580642	25.165248
153.848014	5495.490146	25.170266
154.359540	5499.088628	25.175283
154.555420	5497.569242	25.180301
154.747782	5518.269338	25.185319
155.182424	5531.618930	25.190336
155.117876	5533.721825	25.195354
154.711123	5540.993809	25.200371
155.272837	5543.114899	25.205389
155.291442	5562.933396	25.210407
155.715084	5549.616792	25.215424
155.844315	5559.547079	25.220442
155.792991	5562.005324	25.225459
156.264028	5582.351147	25.230477
156.415770	5603.100987	25.235495
156.684505	5594.757917	25.240512
156.583822	5602.219944	25.245530
156.726937	5612.782316	25.250547
156.871854	5619.976178	25.255565
156.801592	5609.067462	25.260583
157.268980	5620.288964	25.265600
157.464794	5643.409883	25.270618
157.487127	5658.855968	25.275635
157.809998	5658.347630	25.280653
157.597556	5656.383413	25.285671
157.979036	5669.676149	25.290688
157.908869	5674.873770	25.295706
158.467920	5682.640277	25.300723
158.553415	5695.110941	25.305741
158.100749	5723.819496	25.310759
158.353304	5715.459348	25.315776
158.571171	5723.013703	25.320794
158.254192	5733.817557	25.325811
158.638555	5751.347558	25.330829
159.070524	5764.621007	25.335847
159.557685	5781.582001	25.340864
160.070973	5771.065808	25.345882
160.538405	5784.783093	25.350899
160.967049	5776.017380	25.355917
160.976610	5775.763201	25.360935
161.235114	5756.484568	25.365952
161.677706	5766.736890	25.370970
161.965729	5772.518769	25.375987
162.010664	5765.510431	25.381005
161.676668	5750.784740	25.386023
161.782034	5734.424017	25.391040
162.045958	5742.305470	25.396058
161.897907	5752.704989	25.401075
161.809717	5754.935067	25.406093
161.820017	5767.582806	25.411111
162.163675	5763.633479	25.416128
162.003318	5768.779092	25.421146
161.885940	5779.545273	25.426163
162.331797	5784.535601	25.431181
162.253406	5792.631144	25.436199
162.448628	5804.870346	25.441216
162.615004	5820.664504	25.446234
162.806260	5831.901069	25.451251
163.206670	5849.353713	25.456269
162.839663	5863.609006	25.461287
163.654750	5853.104320	25.466304
163.674985	5863.764343	25.471322
163.435943	5887.114190	25.476339
163.825717	5902.837655	25.481357
163.848776	5910.812542	25.486375
163.978467	5917.824774	25.491392
164.113147	5923.650946	25.496410
164.108343	5947.711913	25.501427
164.928319	5946.697738	25.506445
164.611615	5965.670024	25.511463
164.932077	5974.887364	25.516480
165.349899	5980.622672	25.521498
165.547765	6007.660998	25.526515
165.838494	5992.783030	25.531533
165.752421	6009.648401	25.536551
166.136806	6023.986023	25.541568
166.202419	6028.030419	25.546586
166.531044	6043.366421	25.551603
166.763041	6041.636649	25.556621
166.603017	6046.589351	25.561639
166.855848	6053.126887	25.566656
167.397168	6066.453404	25.571674
167.212920	6077.198548	25.576691
167.706416	6069.937975	25.581709
167.705978	6091.527136	25.586727
167.823668	6094.421007	25.591744
168.348727	6089.371357	25.596762
168.049156	6090.978810	25.601779
168.355233	6099.057451	25.606797
168.660566	6115.274695	25.611815
168.733009	6115.664570	25.616832
169.076616	6114.999222	25.621850
169.174522	6131.618539	25.626867
169.569900	6133.137949	25.631885
169.595612	6152.708333	25.636903
169.634924	6137.968637	25.641920
169.552800	6143.430640	25.646938
169.959201	6152.468501	25.651955
170.122233	6163.462679	25.656973
170.050851	6158.065016	25.661991
170.330635	6167.429374	25.667008
170.715224	6170.002732	25.672026
170.512603	6184.362674	25.677044
170.840267	6196.068392	25.682061
170.831464	6197.509681	25.687079
170.852950	6221.890405	25.692096
171.485309	6222.216909	25.697114
171.659209	6225.032213	25.702132
171.949992	6240.999188	25.707149
172.094857	6251.479796	25.712167
173.010125	6240.622020	25.717184
172.943233	6227.463862	25.722202
173.406584	6229.575314	25.727220
173.349829	6224.639865	25.732237
173.377069	6231.379347	25.737255
173.446519	6235.350708	25.742272
173.916285	6234.754292	25.747290
173.560149	6240.152133	25.752308
173.764768	6236.580847	25.757325
173.521325	6237.579715	25.762343
173.657981	6235.960969	25.767360
174.462694	6254.639634	25.772378
173.886074	6257.264717	25.777396
174.120970	6270.597148	25.782413
174.476963	6252.138969	25.787431
174.696072	6258.799508	25.792448
175.196982	6270.294733	25.797466
175.399265	6288.110587	25.802484
175.429829	6284.079766	25.807501
175.382098	6282.359172	25.812519
175.667474	6271.792886	25.817536
175.912743	6266.543693	25.822554
175.698841	6291.931319	25.827572
175.937229	6300.615064	25.832589
175.864392	6306.341782	25.837607
176.053034	6321.881536	25.842624
176.379210	6332.991424	25.847642
176.475150	6343.673917	25.852660
176.753091	6353.297009	25.857677
177.124626	6363.881214	25.862695
177.340356	6368.019028	25.867712
177.317718	6370.026509	25.872730
177.161174	6394.866923	25.877748
177.764112	6399.016374	25.882765
178.038967	6417.142494	25.887783
177.968972	6423.660282	25.892800
178.419423	6428.129483	25.897818
178.403660	6432.785186	25.902836
178.683018	6445.048001	25.907853
178.479970	6455.258605	25.912871
178.905543	6473.522125	25.917888
179.093066	6484.710160	25.922906
179.330182	6483.536302	25.927924
179.680389	6495.213318	25.932941
179.466081	6511.010426	25.937959
179.685899	6514.376579	25.942976
180.017347	6526.752136	25.947994
180.429100	6543.016033	25.953012
180.386480	6540.560555	25.958029
180.712684	6544.948723	25.963047
180.993527	6561.340589	25.968064
181.182079	6572.566319	25.973082
181.418693	6581.717540	25.978100
181.647791	6579.950387	25.983117
181.900935	6592.741381	25.988135
181.598377	6594.056402	25.993152
181.817239	6590.589792	25.998170
182.099309	6605.762348	26.003188
182.455007	6616.776989	26.008205
182.450550	6622.467322	26.013223
182.486432	6638.743804	26.018240
182.836706	6643.317826	26.023258
182.767822	6662.490212	26.028276
182.811886	6674.974800	26.033293
183.089778	6688.194160	26.038311
183.103392	6696.460833	26.043328
183.678543	6719.799461	26.048346
184.401836	6726.470617	26.053364
184.422721	6728.820636	26.058381
184.612211	6744.684361	26.063399
184.449233	6738.472315	26.068416
185.269690	6743.891720	26.073434
185.366386	6745.469205	26.078452
185.080833	6749.693095	26.083469
185.616202	6765.116931	26.088487
185.281553	6776.800989	26.093504
185.569738	6777.619118	26.098522
185.524331	6790.220965	26.103540
185.826748	6808.038189	26.108557
186.139918	6817.212340	26.113575
186.396762	6825.044315	26.118592
186.726399	6830.304634	26.123610
186.634064	6839.115778	26.128628
186.495732	6845.591475	26.133645
186.896196	6854.445643	26.138663
186.905103	6870.800854	26.143680
187.471523	6865.639378	26.148698
187.430822	6888.957149	26.153716
187.759324	6896.895458	26.158733
187.666464	6898.532631	26.163751
187.854540	6923.557938	26.168768
188.410895	6916.440174	26.173786
188.592129	6934.622527	26.178804
188.515303	6955.626927	26.183821
188.934481	6959.717895	26.188839
188.786315	6969.299932	26.193856
189.168968	6972.959827	26.198874
189.095942	6991.394540	26.203892
189.357037	7005.221021	26.208909
190.340184	7010.537244	26.213927
190.480946	7005.907579	26.218944
191.052584	7007.836643	26.223962
191.269990	6998.307331	26.228980
191.083733	6995.484871	26.233997
191.157335	7026.321964	26.239015
191.469837	7027.281005	26.244032
192.273098	7024.706958	26.249050
192.125335	7031.443406	26.254068
192.226048	7030.766175	26.259085
192.632316	7028.616073	26.264103
192.328499	7032.127923	26.269120
192.251389	7028.700669	26.274138
192.753522	7037.468835	26.279156
192.783658	7050.026117	26.284173
192.739066	7055.972115	26.289191
192.888405	7068.626280	26.294208
193.212589	7071.331847	26.299226
192.853202	7085.097886	26.304244
193.378820	7115.972308	26.309261
193.404963	7111.312720	26.314279
193.575818	7137.261908	26.319296
193.873227	7151.216409	26.324314
194.046285	7156.618485	26.329332
194.378845	7185.201533	26.334349
194.580183	7188.870172	26.339367
194.385864	7204.631591	26.344384
194.896615	7209.912520	26.349402
195.150518	7240.388662	26.354420
195.548876	7247.684741	26.359437
195.622229	7253.723165	26.364455
195.716838	7283.650761	26.369472
196.122559	7286.804429	26.374490
196.420236	7288.249525	26.379508
196.348116	7306.899471	26.384525
196.613699	7316.176288	26.389543
196.858566	7331.024896	26.394560
197.021263	7336.832788	26.399578
197.020569	7350.206634	26.404596
197.305844	7363.434006	26.409613
197.899222	7369.111680	26.414631
197.810895	7383.632612	26.419648
198.241327	7393.655668	26.424666
198.346807	7404.883903	26.429684
198.395807	7401.609006	26.434701
198.759501	7405.980196	26.439719
198.871605	7425.977372	26.444736
199.529812	7413.119005	26.449754
199.502452	7426.100367	26.454772
199.887320	7449.071413	26.459789
199.868048	7455.534775	26.464807
200.209946	7455.644669	26.469824
200.226825	7450.680130	26.474842
200.283036	7455.605421	26.479860
200.367114	7457.827753	26.484877
200.953900	7474.785934	26.489895
200.776757	7482.678128	26.494912
200.902985	7481.914751	26.499930
200.938271	7499.420106	26.504948
201.224520	7523.292043	26.509965
201.406144	7518.277423	26.514983
201.215295	7536.737752	26.520000
201.893844	7536.736891	26.525018
201.752331	7558.215110	26.530036
202.172809	7570.905216	26.535053
202.753358	7594.452970	26.540071
202.854821	7600.298642	26.545088
202.739624	7615.685880	26.550106
203.030458	7631.978758	26.555124
202.969336	7642.250164	26.560141
203.512777	7651.906586	26.565159
203.609841	7678.759653	26.570176
203.688615	7689.021365	26.575194
204.254111	7694.588773	26.580212
204.372676	7715.320886	26.585229
204.692456	7724.733125	26.590247
204.801043	7742.096679	26.595264
204.923236	7761.156913	26.600282
204.980187	7770.699243	26.605300
205.040653	7789.260116	26.610317
205.719208	7791.187368	26.615335
205.886008	7809.277810	26.620352
205.983153	7832.823087	26.625370
205.950109	7839.752795	26.630388
206.290111	7858.373106	26.635405
206.892124	7865.998134	26.640423
207.028282	7889.082586	26.645440
206.944230	7900.944239	26.650458
207.478019	7899.428264	26.655476
208.090678	7896.348410	26.660493
208.397867	7897.756549	26.665511
208.478395	7898.989476	26.670528
208.899497	7912.035764	26.675546
208.950020	7910.283006	26.680564
209.006542	7933.227091	26.685581
209.336026	7930.501195	26.690599
209.528479	7936.502874	26.695616
209.180647	7935.260156	26.700634
209.260886	7947.768127	26.705652
209.221759	7967.102580	26.710669
209.472428	7995.502140	26.715687
209.414301	8006.011153	26.720704
209.806815	8027.314346	26.725722
210.289811	8040.934943	26.730740
210.140282	8066.898421	26.735757
210.622318	8074.325984	26.740775
210.854622	8087.204337	26.745792
211.026184	8100.001370	26.750810
211.430860	8107.663847	26.755828
211.549122	8125.994237	26.760845
212.262089	8139.891193	26.765863
212.608918	8145.319246	26.770880
213.556129	8134.213896	26.775898
213.937969	8119.429937	26.780916
213.832183	8116.404944	26.785933
214.010380	8125.528121	26.790951
214.013502	8121.647080	26.795968
214.151939	8126.943364	26.800986
214.210084	8118.744033	26.806004
214.108876	8135.876458	26.811021
214.565878	8131.206032	26.816039
214.555967	8151.215619	26.821056
214.702182	8160.666247	26.826074
215.049206	8163.257174	26.831092
215.215617	8160.276204	26.836109
215.504927	8173.493349	26.841127
215.452955	8189.338560	26.846144
215.536688	8187.313271	26.851162
215.630271	8205.109868	26.856180
215.680514	8230.560142	26.861197
216.011099	8230.965706	26.866215
216.019296	8252.865152	26.871232
216.128778	8270.797821	26.876250
216.751211	8284.193953	26.881268
216.581144	8297.598158	26.886285
216.949311	8319.479179	26.891303
217.072153	8333.746336	26.896320
217.349767	8359.590097	26.901338
217.183948	8381.856375	26.906356
216.974634	8403.723438	26.911373
217.490242	8420.877922	26.916391
217.693839	8452.085417	26.921408
218.104093	8472.041742	26.926426
218.388339	8494.215701	26.931444
218.897540	8515.347466	26.936461
219.344804	8531.189300	26.941479
219.638895	8546.737452	26.946496
220.486778	8537.008533	26.951514
221.085095	8560.194042	26.956532
220.854037	8578.978865	26.961549
221.269348	8574.710608	26.966567
221.233907	8571.242265	26.971584
221.252593	8565.773760	26.976602
221.581279	8586.287983	26.981620
221.524187	8611.482493	26.986637
221.563127	8607.521375	26.991655
222.050656	8632.176965	26.996672
221.919212	8640.287455	27.001690
222.214406	8649.708246	27.006708
221.982637	8672.755381	27.011725
222.016638	8701.142379	27.016743
222.656202	8719.538558	27.021760
223.115484	8734.401107	27.026778
223.306272	8743.270503	27.031796
223.450879	8763.775985	27.036813
223.787642	8786.404829	27.041831
224.040006	8810.678143	27.046848
223.967909	8824.177667	27.051866
224.335851	8827.618305	27.056884
224.681354	8857.089949	27.061901
224.872793	8872.944459	27.066919
225.397398	8888.298901	27.071936
225.430664	8908.875740	27.076954
225.721297	8916.929239	27.081972
226.045155	8927.559279	27.086989
226.072458	8943.144809	27.092007
226.488960	8962.592663	27.097024
226.723867	8972.200048	27.102042
227.210930	8982.923678	27.107060
227.222464	8987.017152	27.112077
227.786217	8985.785212	27.117095
228.007504	9003.281186	27.122112
228.192527	9011.330127	27.127130
228.539944	9014.006989	27.132148
228.496017	9023.394235	27.137165
228.592058	9045.448035	27.142183
229.168349	9045.946149	27.147200
229.062797	9038.725707	27.152218
229.434226	9043.276459	27.157236
229.262814	9065.075152	27.162253
229.435747	9079.967218	27.167271
229.861832	9088.734917	27.172288
230.014598	9110.913344	27.177306
229.941293	9122.096715	27.182324
230.208712	9137.282000	27.187341
230.293069	9151.538133	27.192359
230.943422	9157.142456	27.197376
231.015396	9183.786386	27.202394
231.026253	9204.846229	27.207412
231.052304	9222.329802	27.212429
231.577557	9241.515844	27.217447
232.229878	9252.754290	27.222464
232.114984	9273.393101	27.227482
232.742870	9276.070144	27.232500
233.172102	9289.963794	27.237517
233.622512	9298.551145	27.242535
233.792697	9308.369503	27.247552
233.755559	9307.469978	27.252570
234.103343	9316.619385	27.257588
234.412091	9322.753616	27.262605
234.309574	9322.406044	27.267623
234.942844	9349.135536	27.272640
234.940741	9368.792472	27.277658
234.922409	9367.450297	27.282676
234.973701	9384.628187	27.287693
235.278571	9393.451528	27.292711
235.925509	9408.087567	27.297728
235.932690	9426.746591	27.302746
236.321161	9444.710898	27.307764
236.618522	9465.872628	27.312781
236.518535	9469.339516	27.317799
236.845093	9484.837536	27.322816
236.695146	9495.461953	27.327834
237.332986	9515.281950	27.332852
237.568007	9531.117314	27.337869
237.475188	9541.896167	27.342887
238.033509	9570.944054	27.347904
238.093837	9584.633450	27.352922
238.074526	9597.846055	27.357940
238.712304	9616.493279	27.362957
238.607803	9636.362816	27.367975
238.950148	9653.451160	27.372992
239.102774	9671.393246	27.378010
239.566352	9683.644683	27.383028
240.221078	9717.110203	27.388045
240.221752	9726.183282	27.393063
240.835555	9727.292011	27.398080
240.523268	9745.416547	27.403098
241.183787	9752.258495	27.408116
241.317382	9758.870049	27.413133
241.680880	9782.811394	27.418151
241.913800	9790.043034	27.423168
242.014812	9803.304462	27.428186
242.219964	9800.326242	27.433204
242.804044	9820.658072	27.438221
242.810248	9836.017944	27.443239
243.073118	9845.057224	27.448256
243.097298	9871.117825	27.453274
243.493342	9868.709092	27.458292
243.607392	9887.082381	27.463309
243.809782	9902.001859	27.468327
244.397113	9914.865577	27.473344
244.235851	9926.683200	27.478362
244.668007	9926.947573	27.483380
244.729547	9938.804805	27.488397
245.225905	9957.205601	27.493415
245.399193	9963.616900	27.498432
245.464685	9987.978812	27.503450
245.558845	10001.421928	27.508468
245.919482	10012.817026	27.513485
246.071356	10015.649255	27.518503
245.938157	10031.490021	27.523520
246.166900	10059.727526	27.528538
246.506950	10080.954704	27.533556
246.721494	10094.998750	27.538573
246.955719	10115.887399	27.543591
247.571083	10144.319557	27.548608
247.870147	10146.991212	27.553626
248.389238	10180.698320	27.558644
248.338841	10182.027893	27.563661
248.592938	10192.577352	27.568679
248.991618	10210.424251	27.573696
249.232543	10222.759366	27.578714
249.711046	10232.526568	27.583732
249.462153	10253.088736	27.588749
249.856386	10263.329137	27.593767
250.240293	10284.115290	27.598784
250.921513	10306.518444	27.603802
250.991051	10312.319973	27.608820
251.696267	10320.049671	27.613837
251.912433	10325.907331	27.618855
252.150883	10314.582004	27.623872
252.092026	10326.814691	27.628890
252.897848	10325.590718	27.633908
253.149554	10347.744277	27.638925
253.092856	10346.503676	27.643943
253.660624	10343.467022	27.648960
253.443680	10343.351025	27.653978
253.519702	10359.734973	27.658996
253.975277	10380.666962	27.664013
254.257663	10384.712894	27.669031
254.617018	10400.311159	27.674048
254.041608	10420.765209	27.679066
254.458700	10434.327856	27.684084
254.922022	10450.539199	27.689101
255.026326	10470.621055	27.694119
254.932681	10475.941499	27.699136
255.244072	10510.970032	27.704154
255.680558	10515.875983	27.709172
255.928855	10546.709157	27.714189
255.737388	10568.565990	27.719207
256.190569	10584.526272	27.724224
256.339447	10608.491710	27.729242
256.731390	10616.488371	27.734260
257.211113	10642.295354	27.739277
257.297231	10673.992177	27.744295
257.718599	10683.958161	27.749312
257.753430	10718.756332	27.754330
258.036008	10730.175869	27.759348
258.448775	10746.799992	27.764365
258.734757	10779.844183	27.769383
259.073019	10780.229649	27.774400
259.498831	10811.846201	27.779418
259.346497	10828.925362	27.784436
260.277629	10845.775908	27.789453
260.024477	10856.507295	27.794471
260.576111	10866.474717	27.799488
260.825329	10890.503565	27.804506
261.172032	10906.481760	27.809524
261.335755	10901.266582	27.814541
261.464839	10930.680126	27.819559
261.779062	10943.583496	27.824576
262.027682	10964.694606	27.829594
262.344782	10975.153032	27.834612
262.596348	10978.729962	27.839629
262.574760	11002.404311	27.844647
262.724559	11010.316704	27.849664
263.177967	11038.398287	27.854682
263.308034	11054.847281	27.859700
263.728768	11065.160235	27.864717
263.789881	11100.633965	27.869735
264.140974	11112.839700	27.874752
264.695799	11122.138708	27.879770
264.791092	11134.201589	27.884788
265.454189	11148.126762	27.889805
265.562847	11175.971696	27.894823
265.871090	11187.744190	27.899840
265.718210	11201.497766	27.904858
265.953547	11221.063389	27.909876
266.387259	11227.666146	27.914893
266.044152	11263.080969	27.919911
266.518977	11287.104649	27.924928
267.098288	11310.969300	27.929946
267.161985	11331.689970	27.934964
267.980561	11333.254218	27.939981
268.242654	11355.968369	27.944999
268.653489	11371.096635	27.950016
268.471846	11385.381373	27.955034
268.745787	11400.348724	27.960052
269.467401	11420.974995	27.965069
269.638379	11443.362415	27.970087
269.980607	11450.525542	27.975104
270.553092	11471.359287	27.980122
270.203691	11488.240088	27.985140
270.868946	11490.319701	27.990157
270.843178	11513.630737	27.995175
271.156840	11530.279926	28.000192
271.733609	11540.484689	28.005210
272.032870	11553.129468	28.010228
272.301800	11550.189235	28.015245
272.380694	11571.801872	28.020263
273.083266	11583.039973	28.025280
273.028206	11599.075781	28.030298
273.023533	11627.412909	28.035316
273.735623	11634.437807	28.040333
273.276771	11657.710307	28.045351
273.736873	11661.984034	28.050368
274.051110	11677.452341	28.055386
274.549180	11694.671553	28.060404
275.068304	11719.213251	28.065421
275.109644	11742.883807	28.070439
275.208591	11755.479119	28.075456
275.480790	11762.580688	28.080474
275.497202	11787.668783	28.085492
276.004733	11798.531953	28.090509
276.029909	11830.111921	28.095527
276.676398	11844.717188	28.100544
277.048514	11871.988017	28.105562
277.022200	11890.066932	28.110580
277.140767	11897.489378	28.115597
277.233471	11931.982812	28.120615
277.792446	11955.788756	28.125632
278.103012	11980.339310	28.130650
278.379825	11997.038401	28.135668
278.645248	12009.632407	28.140685
279.172010	12030.913257	28.145703
279.556354	12051.463704	28.150720
279.914413	12052.849640	28.155738
280.144069	12071.170090	28.160756
280.490605	12085.870040	28.165773
280.616571	12083.363007	28.170791
280.705319	12101.531083	28.175808
281.384888	12118.659313	28.180826
281.322030	12132.795881	28.185844
281.765232	12140.386978	28.190861
281.659964	12160.743496	28.195879
282.415739	12176.894092	28.200896
282.825270	12173.962033	28.205914
283.011471	12194.034087	28.210932
283.517428	12200.620586	28.215949
283.626648	12210.096267	28.220967
284.019153	12236.793159	28.225984
284.285938	12228.842457	28.231002
284.319415	12251.355350	28.236020
284.506948	12263.033551	28.241037
284.330068	12285.702573	28.246055
285.027386	12305.616268	28.251072
285.422282	12324.551017	28.256090
285.313637	12347.788711	28.261108
285.714002	12362.263361	28.266125
285.445512	12390.437421	28.271143
285.447110	12415.970138	28.276160
286.266941	12442.239085	28.281178
286.544629	12474.854808	28.286196
286.921035	12487.370188	28.291213
287.311198	12529.744766	28.296231
287.362512	12540.222913	28.301248
288.323897	12573.661862	28.306266
288.320755	12592.984134	28.311284
288.805927	12599.517505	28.316301
289.110772	12614.911056	28.321319
289.200505	12630.639548	28.326336
289.707883	12644.988047	28.331354
289.941815	12679.174539	28.336372
290.056601	12694.574352	28.341389
290.274691	12718.642588	28.346407
290.654414	12735.711500	28.351424
291.051171	12762.050865	28.356442
291.158848	12787.585553	28.361460
291.886970	12802.967657	28.366477
291.715328	12826.616685	28.371495
292.014657	12847.825887	28.376512
292.528578	12872.365476	28.381530
292.786523	12894.730302	28.386548
293.224833	12922.857851	28.391565
293.629811	12931.010306	28.396583
293.531156	12942.295066	28.401600
294.257951	12958.747480	28.406618
294.908526	12960.893539	28.411636
295.416459	12972.834474	28.416653
295.607339	12998.595265	28.421671
295.908794	12997.459956	28.426688
296.201086	13005.104759	28.431706
296.221687	13028.953960	28.436724
296.558815	13027.346328	28.441741
296.565856	13066.958680	28.446759
297.113254	13066.948808	28.451776
297.797493	13069.131866	28.456794
298.165005	13091.653774	28.461812
298.638343	13078.849813	28.466829
298.409758	13078.741226	28.471847
298.906687	13096.846927	28.476864
298.989474	13098.551043	28.481882
298.957693	13122.676919	28.486900
299.411586	13121.478599	28.491917
299.615591	13143.307462	28.496935
299.643269	13171.744379	28.501952
299.931448	13174.150462	28.506970
299.959214	13207.235989	28.511988
300.057069	13216.408436	28.517005
300.597687	13231.153794	28.522023
300.751970	13266.451434	28.527040
301.096980	13281.936685	28.532058
301.126148	13318.321921	28.537076
301.594076	13334.136742	28.542093
302.216675	13361.812296	28.547111
302.291051	13380.728750	28.552128
302.841741	13403.186163	28.557146
302.891472	13425.638123	28.562164
303.482987	13452.579914	28.567181
304.158279	13461.661831	28.572199
304.582355	13480.467052	28.577216
305.072627	13486.045001	28.582234
304.887111	13516.664002	28.587252
305.100675	13521.468252	28.592269
305.332238	13545.885324	28.597287
305.637886	13558.195762	28.602304
306.643312	13579.609166	28.607322
306.485215	13593.239568	28.612340
306.659837	13624.839320	28.617357
306.906668	13635.057380	28.622375
307.007669	13651.906993	28.627392
307.715759	13670.320407	28.632410
307.568523	13699.385961	28.637428
307.684602	13721.936102	28.642445
308.072180	13755.391932	28.647463
308.142259	13780.345030	28.652480
308.611366	13808.757412	28.657498
308.631107	13833.914314	28.662516
308.947739	13855.266956	28.667533
309.395668	13888.661087	28.672551
309.461607	13940.618956	28.677568
310.056744	13975.982407	28.682586
310.070640	13998.195244	28.687604
310.537916	14023.491246	28.692621
311.348709	14052.485832	28.697639
311.438024	14086.409222	28.702656
312.174923	14102.982479	28.707674
312.660259	14128.672782	28.712692
312.974394	14144.252207	28.717709
313.267432	14173.617779	28.722727
313.457544	14192.922636	28.727744
314.161632	14197.349785	28.732762
314.488329	14220.054928	28.737780
314.628932	14232.564916	28.742797
315.232578	14249.645711	28.747815
315.236573	14271.551682	28.752832
315.732217	14292.002282	28.757850
315.758739	14315.338653	28.762868
316.243294	14332.819000	28.767885
316.924962	14340.614431	28.772903
317.115313	14358.447558	28.777920
317.399647	14370.554116	28.782938
317.014479	14404.640079	28.787956
317.406254	14436.716127	28.792973
317.863629	14447.222977	28.797991
317.884562	14477.275444	28.803008
318.453663	14488.186207	28.808026
318.311479	14528.721890	28.813044
318.318865	14554.420908	28.818061
318.836793	14590.082117	28.823079
318.911534	14630.626341	28.828096
319.697975	14638.212345	28.833114
319.863653	14684.344097	28.838132
320.281164	14699.924312	28.843149
321.215299	14714.189967	28.848167
321.525846	14743.684478	28.853184
321.905263	14757.182927	28.858202
322.449423	14773.530259	28.863220
322.419683	14792.008532	28.868237
322.536296	14793.034312	28.873255
322.484167	14824.065540	28.878272
323.418810	14843.960497	28.883290
324.180716	14865.787760	28.888308
324.190379	14879.746110	28.893325
324.771985	14896.782373	28.898343
324.869875	14907.998202	28.903360
325.369821	14918.307635	28.908378
325.543308	14949.747824	28.913396
325.398469	14957.935400	28.918413
326.049996	14977.008941	28.923431
325.977648	14994.974416	28.928448
326.585058	15019.014841	28.933466
326.789548	15048.138161	28.938484
326.722940	15079.414963	28.943501
327.483087	15093.087189	28.948519
327.495318	15127.397409	28.953536
327.855672	15144.760463	28.958554
328.184100	15187.054466	28.963572
328.553589	15216.735516	28.968589
328.959747	15232.325998	28.973607
329.006470	15266.367621	28.978624
329.364546	15283.360842	28.983642
329.456109	15328.570520	28.988660
329.806779	15354.073822	28.993677
330.306159	15388.390791	28.998695
330.168856	15443.527984	29.003712
330.674336	15463.021799	29.008730
331.078216	15498.339777	29.013748
331.403520	15524.963350	29.018765
332.214019	15554.723456	29.023783
332.145161	15594.192159	29.028800
332.707602	15628.508670	29.033818
333.563696	15660.009243	29.038836
333.622341	15681.572382	29.043853
334.531401	15710.022572	29.048871
334.834178	15734.743213	29.053888
335.207550	15747.561061	29.058906
335.194025	15767.626397	29.063924
335.444969	15803.736253	29.068941
336.133194	15812.086080	29.073959
336.204455	15839.098861	29.078976
336.552190	15857.110935	29.083994
336.971444	15878.249118	29.089012
336.960111	15911.102301	29.094029
337.393071	15930.137416	29.099047
337.608838	15967.236899	29.104064
337.851998	15982.451555	29.109082
338.378913	16019.906377	29.114100
338.970340	16042.874504	29.119117
339.586027	16065.455672	29.124135
339.807681	16090.609485	29.129152
340.055997	16105.353736	29.134170
340.600003	16130.960276	29.139188
340.319816	16152.483869	29.144205
341.222339	16173.192710	29.149223
341.104275	16205.868682	29.154240
341.680163	16234.054882	29.159258
342.008104	16262.617797	29.164276
342.319134	16290.805294	29.169293
342.862268	16319.659008	29.174311
342.940187	16343.924400	29.179328
342.931258	16370.743259	29.184346
343.329461	16387.117899	29.189364
343.453686	16407.736535	29.194381
344.134347	16429.831492	29.199399
344.179904	16461.183812	29.204416
344.248311	16481.999318	29.209434
344.811257	16513.701271	29.214452
345.295704	16550.618989	29.219469
345.644046	16570.455306	29.224487
345.907670	16614.973409	29.229504
346.141829	16637.943074	29.234522
346.559584	16672.079203	29.239540
347.101732	16687.295556	29.244557
347.489564	16720.993839	29.249575
347.604058	16747.110460	29.254592
348.343670	16782.794994	29.259610
348.427897	16823.508570	29.264628
348.668600	16852.041213	29.269645
349.506112	16872.268350	29.274663
349.503100	16920.268888	29.279680
349.947207	16946.552034	29.284698
350.438673	16950.687236	29.289716
351.439992	16970.772376	29.294733
351.909423	16978.314133	29.299751
351.789041	17002.368951	29.304768
352.181566	17028.496830	29.309786
352.861921	17051.431191	29.314804
353.019205	17075.247954	29.319821
353.389751	17086.030920	29.324839
353.504577	17107.025535	29.329856
353.968062	17137.302934	29.334874
354.238689	17169.480008	29.339892
353.935583	17194.432185	29.344909
354.926443	17218.114603	29.349927
355.051300	17236.674115	29.354944
355.193082	17275.208905	29.359962
355.985208	17303.958593	29.364980
356.236702	17339.926725	29.369997
356.599395	17365.650259	29.375015
356.964540	17392.606009	29.380032
357.544601	17406.899426	29.385050
358.069068	17430.935032	29.390068
358.555039	17459.864817	29.395085
359.212699	17482.450461	29.400103
359.176425	17500.294499	29.405120
359.896271	17521.344162	29.410138
360.098268	17528.471678	29.415156
359.969303	17551.964434	29.420173
360.603589	17573.764387	29.425191
360.991507	17592.071207	29.430208
361.263841	17618.169438	29.435226
361.210315	17633.439364	29.440244
361.588388	17672.886505	29.445261
361.720437	17694.115455	29.450279
361.897057	17724.860597	29.455296
362.393571	17757.453879	29.460314
362.803749	17798.191672	29.465332
362.534078	17849.030463	29.470349
362.884162	17879.205012	29.475367
363.474732	17922.753691	29.480384
363.639617	17956.606396	29.485402
364.699584	17984.945764	29.490420
365.033772	18033.309962	29.495437
365.029042	18068.603237	29.500455
365.187067	18109.821652	29.505472
365.906782	18132.866086	29.510490
367.273537	18145.299454	29.515508
367.684278	18159.200635	29.520525
368.494478	18166.721326	29.525543
368.583130	18190.380799	29.530560
368.826377	18208.406407	29.535578
369.091292	18215.298421	29.540596
369.334780	18241.575791	29.545613
369.655572	18245.484164	29.550631
369.739857	18280.548814	29.555648
369.721059	18303.657164	29.560666
370.244167	18344.171156	29.565684
370.515692	18365.139908	29.570701
371.190789	18382.599413	29.575719
371.172204	18411.765540	29.580736
371.005370	18454.018927	29.585754
371.632124	18483.787905	29.590772
371.936782	18528.421036	29.595789
372.545342	18558.163204	29.600807
372.833253	18591.483010	29.605824
372.741793	18636.464026	29.610842
373.166493	18670.715061	29.615860
373.336325	18720.062084	29.620877
374.004105	18752.774056	29.625895
374.516393	18781.626146	29.630912
374.936876	18829.133503	29.635930
375.523616	18862.122325	29.640948
375.799621	18914.925042	29.645965
376.531606	18952.792454	29.650983
376.667969	18985.691982	29.656000
377.360496	19022.888246	29.661018
377.760372	19037.815009	29.666036
377.740401	19094.128846	29.671053
378.354753	19121.033635	29.676071
378.909428	19151.414735	29.681088
379.281198	19187.554599	29.686106
380.063679	19214.986646	29.691124
380.308356	19247.306038	29.696141
380.696870	19268.450500	29.701159
381.006171	19297.940769	29.706176
381.425537	19330.576691	29.711194
382.078671	19357.929455	29.716212
382.082776	19388.773965	29.721229
382.395756	19419.075677	29.726247
382.790595	19453.779377	29.731264
383.403519	19481.282437	29.736282
384.151972	19498.399964	29.741300
384.654414	19528.818759	29.746317
384.904188	19544.492763	29.751335
385.392346	19568.638366	29.756352
385.416969	19603.972616	29.761370
386.161590	19624.197990	29.766388
385.919783	19652.711127	29.771405
386.366631	19672.443467	29.776423
386.606775	19705.902664	29.781440
386.760440	19752.009591	29.786458
387.131069	19788.790974	29.791476
387.452858	19820.280580	29.796493
387.997876	19854.651330	29.801511
388.234926	19893.282085	29.806528
388.591435	19924.818175	29.811546
389.588059	19958.121386	29.816564
389.755708	19993.735510	29.821581
390.008101	20024.916949	29.826599
390.536669	20063.165736	29.831616
390.552500	20092.679092	29.836634
391.095715	20134.584555	29.841652
391.288063	20182.398306	29.846669
391.828115	20207.242514	29.851687
392.120979	20242.844367	29.856704
392.024123	20279.716669	29.861722
392.991763	20319.952375	29.866740
393.675960	20345.307401	29.871757
394.307152	20367.850913	29.876775
395.234977	20385.305467	29.881792
395.333353	20403.352659	29.886810
396.211584	20398.632849	29.891828
396.689625	20419.332032	29.896845
397.142942	20434.892850	29.901863
397.975205	20439.204388	29.906880
398.318394	20454.578475	29.911898
398.922248	20454.746923	29.916916
399.141496	20465.966975	29.921933
398.927978	20464.195795	29.926951
399.674877	20487.287890	29.931968
399.582806	20519.936533	29.936986
399.870327	20533.659849	29.942004
399.712871	20552.730039	29.947021
400.112870	20587.660687	29.952039
400.499376	20614.474684	29.957056
400.189127	20652.678938	29.962074
400.627722	20673.329775	29.967092
401.053125	20722.905361	29.972109
400.847155	20766.495333	29.977127
401.634116	20814.105464	29.982144
401.873924	20862.949090	29.987162
402.489350	20907.992875	29.992180
403.121876	20945.800851	29.997197
403.446594	20988.379890	30.002215
403.899882	21022.523837	30.007232
404.398066	21073.690198	30.012250
404.958366	21103.665608	30.017268
405.372317	21148.590397	30.022285
405.463707	21195.742652	30.027303
406.136074	21226.177464	30.032320
406.749570	21262.843146	30.037338
407.181877	21295.759826	30.042356
407.822496	21344.790896	30.047373
408.388264	21382.773273	30.052391
409.175095	21399.842278	30.057408
409.439727	21428.804504	30.062426
410.149729	21454.899520	30.067444
410.512717	21478.770594	30.072461
411.099887	21495.989346	30.077479
411.613925	21509.128972	30.082496
412.226345	21516.340181	30.087514
412.656148	21535.202540	30.092532
412.900830	21547.967321	30.097549
413.348717	21567.676508	30.102567
413.706231	21589.161694	30.107584
413.956393	21620.910895	30.112602
414.492471	21642.478591	30.117620
414.629563	21664.116952	30.122637
414.458859	21682.017625	30.127655
415.070333	21711.741299	30.132672
415.319270	21748.701603	30.137690
415.924147	21786.033604	30.142708
415.896651	21822.796936	30.147725
415.987825	21865.659579	30.152743
416.576348	21892.826946	30.157760
416.510541	21931.149809	30.162778
417.205881	21972.486083	30.167796
417.637273	22033.163981	30.172813
417.746171	22086.195090	30.177831
418.184046	22118.064002	30.182848
418.734096	22166.035590	30.187866
418.960044	22199.699195	30.192884
419.409913	22258.400894	30.197901
419.929548	22301.080349	30.202919
420.547865	22344.085745	30.207936
420.772861	22360.844917	30.212954
421.131352	22405.449553	30.217972
421.834401	22444.233095	30.222989
421.916901	22483.328931	30.228007
422.746962	22524.362083	30.233024
422.813860	22562.683379	30.238042
423.344307	22595.859160	30.243060
423.894960	22639.913946	30.248077
424.068119	22682.400907	30.253095
425.139995	22718.036998	30.258112
425.638314	22758.412855	30.263130
426.133228	22785.597128	30.268148
426.672442	22810.295553	30.273165
426.686371	22846.530808	30.278183
427.273840	22884.930821	30.283200
427.512604	22933.028540	30.288218
428.146180	22970.514523	30.293236
428.324823	22994.326749	30.298253
428.962059	23032.337312	30.303271
429.448776	23066.850420	30.308288
429.895671	23110.636610	30.313306
430.029480	23150.517031	30.318324
430.480111	23186.250428	30.323341
430.878258	23231.448279	30.328359
431.041130	23265.116544	30.333376
432.058104	23305.491603	30.338394
432.384058	23352.995871	30.343412
432.527268	23394.275468	30.348429
432.533753	23439.716745	30.353447
433.415885	23482.372420	30.358464
433.584989	23534.371654	30.363482
434.164863	23570.114472	30.368500
434.729786	23612.556399	30.373517
435.076391	23673.624738	30.378535
435.426631	23719.612311	30.383552
435.807201	23766.564725	30.388570
436.460261	23807.458366	30.393588
436.948647	23847.778547	30.398605
436.787546	23906.952709	30.403623
437.416773	23955.394070	30.408640
437.823521	24004.824714	30.413658
438.953033	24045.042614	30.418676
440.144752	24068.263266	30.423693
440.492598	24099.860654	30.428711
441.120959	24125.058743	30.433728
441.678215	24164.631925	30.438746
442.319938	24201.351376	30.443764
442.349784	24225.126837	30.448781
442.246898	24263.919962	30.453799
442.942054	24289.269675	30.458816
443.211491	24321.096455	30.463834
443.409160	24365.425337	30.468852
444.372825	24394.602011	30.473869
444.661616	24447.382156	30.478887
445.076753	24472.798898	30.483904
445.477740	24514.231014	30.488922
445.682654	24540.245521	30.493940
446.402052	24570.224471	30.498957
446.845410	24616.093441	30.503975
447.263184	24648.057170	30.508992
448.000279	24691.774277	30.514010
447.938343	24720.387677	30.519028
449.054559	24749.576034	30.524045
449.288439	24787.572012	30.529063
449.687328	24825.176556	30.534080
450.036771	24862.846120	30.539098
450.089563	24910.273713	30.544116
450.460069	24932.311342	30.549133
450.883191	24985.873607	30.554151
451.309241	25015.211116	30.559168
451.812172	25042.662608	30.564186
451.725679	25084.222364	30.569204
452.389076	25123.758170	30.574221
452.714679	25170.744040	30.579239
453.266898	25197.263566	30.584256
453.741903	25251.873057	30.589274
454.052642	25290.738962	30.594292
454.652643	25325.630608	30.599309
454.906328	25381.994355	30.604327
455.609631	25422.856776	30.609344
456.164080	25473.943580	30.614362
456.255705	25519.360571	30.619380
456.911215	25561.458088	30.624397
457.300563	25620.731774	30.629415
458.133459	25660.784879	30.634432
459.020235	25698.854813	30.639450
458.995158	25738.018482	30.644468
459.747014	25766.954955	30.649485
459.716626	25818.155161	30.654503
460.387955	25863.761168	30.659520
460.733579	25906.774910	30.664538
461.290128	25944.972481	30.669556
462.127474	25997.468107	30.674573
462.553232	26041.979714	30.679591
462.889898	26074.792170	30.684608
463.788885	26098.071848	30.689626
465.144280	26140.143497	30.694644
465.839487	26168.601138	30.699661
466.276011	26194.420630	30.704679
466.744612	26213.463155	30.709696
467.461086	26218.167521	30.714714
467.711636	26245.793530	30.719732
468.002404	26268.193001	30.724749
468.298581	26298.041466	30.729767
468.658628	26303.268375	30.734784
468.928380	26338.836413	30.739802
469.094906	26361.925188	30.744820
469.716815	26399.784958	30.749837
469.897342	26456.254217	30.754855
470.406291	26477.230128	30.759872
470.379564	26517.935042	30.764890
470.248369	26559.054724	30.769908
470.854011	26606.244299	30.774925
470.922290	26674.119133	30.779943
470.970085	26732.327062	30.784960
471.545585	26789.754111	30.789978
471.750258	26856.093147	30.794996
472.838548	26906.455753	30.800013
473.264524	26973.827948	30.805031
473.453757	27029.565883	30.810048
474.156016	27091.291076	30.815066
474.454441	27153.029575	30.820084
475.143141	27201.784168	30.825101
475.431977	27276.778702	30.830119
476.285974	27328.105432	30.835136
477.204308	27384.285537	30.840154
478.043415	27448.131140	30.845172
478.446104	27489.350956	30.850189
479.125138	27536.653978	30.855207
479.844226	27573.878891	30.860224
480.500977	27604.988556	30.865242
480.798358	27651.566363	30.870260
481.187311	27681.682638	30.875277
481.680594	27733.953365	30.880295
481.950486	27768.707369	30.885312
482.304656	27805.873196	30.890330
482.636565	27848.991848	30.895348
483.332128	27881.814713	30.900365
483.606658	27930.299112	30.905383
483.466916	27977.331675	30.910400
484.000266	28025.259429	30.915418
484.155014	28082.343909	30.920436
484.675882	28130.510595	30.925453
485.296125	28187.591084	30.930471
486.062940	28236.357782	30.935488
486.356743	28284.543476	30.940506
486.668775	28352.523441	30.945524
487.061788	28411.471768	30.950541
487.468146	28480.215798	30.955559
488.199411	28528.263668	30.960576
488.863070	28581.846306	30.965594
489.382503	28638.916546	30.970612
490.250662	28690.614065	30.975629
491.123591	28744.351909	30.980647
491.481875	28784.575865	30.985664
492.501160	28820.441610	30.990682
492.570123	28873.413615	30.995700
493.297364	28916.100548	31.000717
493.791332	28961.807151	31.005735
494.232086	29001.771935	31.010752
494.959095	29030.932523	31.015770
495.369988	29077.350308	31.020788
496.105024	29107.607484	31.025805
496.578706	29155.646015	31.030823
496.615279	29195.592833	31.035840
497.380319	29249.687605	31.040858
497.528520	29307.455434	31.045876
497.924225	29337.781680	31.050893
498.520609	29389.904729	31.055911
498.609724	29442.843594	31.060928
499.200645	29486.642792	31.065946
499.535875	29549.213423	31.070964
500.284332	29602.750508	31.075981
500.676647	29656.904957	31.080999
501.220116	29704.759972	31.086016
501.930611	29745.577839	31.091034
502.376454	29815.866425	31.096052
503.088932	29850.336978	31.101069
504.489575	29877.845079	31.106087
505.192263	29912.793733	31.111104
506.074020	29947.533062	31.116122
506.653886	29980.344317	31.121140
507.258922	29997.693334	31.126157
507.546239	30021.442153	31.131175
507.817449	30047.405132	31.136192
508.678491	30081.460420	31.141210
508.447484	30111.553974	31.146228
508.991905	30142.040034	31.151245
509.545761	30174.360655	31.156263
509.788529	30215.480869	31.161280
510.270949	30257.526955	31.166298
510.606348	30301.039159	31.171316
511.296198	30339.353783	31.176333
511.698701	30378.911618	31.181351
511.768335	30424.979241	31.186368
512.255388	30470.873931	31.191386
512.428545	30520.552734	31.196404
513.160516	30566.590200	31.201421
514.009630	30621.476676	31.206439
514.467572	30670.774456	31.211456
514.565135	30711.569633	31.216474
514.749694	30764.256972	31.221492
515.725646	30794.631883	31.226509
516.510853	30839.547609	31.231527
517.050314	30894.517638	31.236544
517.770602	30932.421557	31.241562
517.898866	30978.597683	31.246580
518.390026	31021.013286	31.251597
518.528658	31065.055212	31.256615
519.163797	31106.639583	31.261632
519.741470	31147.955911	31.266650
520.060977	31205.998289	31.271668
519.966202	31263.901059	31.276685
520.440111	31312.185268	31.281703
521.091882	31379.679232	31.286720
521.638186	31429.734366	31.291738
522.436825	31491.708529	31.296756
522.898356	31551.574261	31.301773
523.808681	31606.251796	31.306791
523.864430	31681.032480	31.311808
524.472115	31725.124788	31.316826
524.888074	31786.983364	31.321844
525.756446	31834.345685	31.326861
526.609636	31897.851938	31.331879
526.845526	31947.679019	31.336896
527.708735	32012.780499	31.341914
527.920285	32056.853882	31.346932
528.654261	32108.747768	31.351949
529.028980	32166.200504	31.356967
529.093631	32228.935833	31.361984
529.967910	32287.183575	31.367002
530.745584	32361.188485	31.372020
531.321085	32407.458561	31.377037
531.934389	32460.010755	31.382055
532.362180	32513.713834	31.387072
532.904171	32557.270079	31.392090
533.384740	32611.813484	31.397108
533.953950	32674.019021	31.402125
534.607569	32728.739292	31.407143
535.130432	32786.917367	31.412160
535.394579	32846.012364	31.417178
535.886454	32907.710885	31.422196
536.517515	32961.649948	31.427213
537.105219	33023.796868	31.432231
537.472850	33082.601056	31.437248
538.148569	33134.681126	31.442266
538.671391	33196.293505	31.447284
539.413443	33256.308012	31.452301
539.763249	33314.181943	31.457319
540.005996	33379.684395	31.462336
540.738630	33441.203021	31.467354
541.171779	33492.895084	31.472372
541.351396	33564.302836	31.477389
541.876283	33626.317101	31.482407
542.618469	33702.602203	31.487424
543.550570	33770.134745	31.492442
544.040966	33830.123344	31.497460
544.330002	33892.095452	31.502477
545.591782	33935.397370	31.507495
545.759790	34017.057689	31.512512
546.525223	34076.354828	31.517530
547.072489	34133.075476	31.522548
547.395929	34185.570232	31.527565
548.085206	34243.684585	31.532583
548.491821	34300.318556	31.537600
549.211311	34365.045383	31.542618
549.182472	34427.314832	31.547636
549.905604	34489.084792	31.552653
550.302973	34544.881699	31.557671
550.992954	34607.380163	31.562688
552.003419	34659.586134	31.567706
552.121993	34729.598115	31.572724
552.779877	34796.182691	31.577741
553.065150	34847.432938	31.582759
553.418188	34911.480713	31.587776
554.094221	34973.572538	31.592794
554.865639	35031.369802	31.597812
555.364829	35098.054296	31.602829
556.026823	35150.126769	31.607847
556.583511	35213.706514	31.612864
556.746052	35272.050071	31.617882
557.258198	35337.480521	31.622900
557.777570	35401.228037	31.627917
558.642624	35458.686184	31.632935
558.936205	35528.991118	31.637952
559.640097	35600.178430	31.642970
560.436539	35665.941814	31.647988
560.922840	35731.100269	31.653005
561.901346	35793.495275	31.658023
562.119125	35844.339812	31.663040
562.726690	35907.850508	31.668058
563.248622	35968.866723	31.673076
564.176099	36038.642929	31.678093
564.840804	36087.464058	31.683111
564.799200	36165.403943	31.688128
565.761259	36223.527028	31.693146
566.738847	36277.456782	31.698164
567.352432	36339.860315	31.703181
568.262083	36381.739945	31.708199
568.871871	36438.246149	31.713216
569.479687	36489.277409	31.718234
570.216054	36534.493377	31.723252
571.064954	36578.838781	31.728269
571.837545	36621.091912	31.733287
571.924821	36669.713342	31.738304
572.696818	36712.074087	31.743322
573.261027	36764.511404	31.748340
573.682883	36824.511914	31.753357
573.948432	36868.812365	31.758375
574.283128	36915.045572	31.763392
575.007351	36970.707692	31.768410
575.624021	37020.820615	31.773428
576.541285	37071.682495	31.778445
577.484671	37119.551483	31.783463
578.134141	37160.873112	31.788480
578.422265	37209.636408	31.793498
579.017301	37248.622318	31.798516
579.532657	37305.150001	31.803533
579.910642	37353.857817	31.808551
580.369212	37411.291524	31.813568
580.460828	37465.008231	31.818586
581.305324	37518.824830	31.823604
581.789278	37579.016429	31.828621
582.507622	37634.855158	31.833639
582.711417	37699.906451	31.838656
583.493928	37744.148921	31.843674
584.704129	37796.106973	31.848692
585.028694	37850.057776	31.853709
585.849964	37911.946418	31.858727
585.764925	37962.730178	31.863744
586.428135	38023.540660	31.868762
587.312086	38073.214691	31.873780
587.686003	38138.021688	31.878797
588.578012	38182.206117	31.883815
588.769190	38230.287509	31.888832
589.138566	38298.144700	31.893850
590.056748	38362.111434	31.898868
590.148499	38425.858235	31.903885
591.317954	38484.200556	31.908903
591.515061	38533.686294	31.913920
591.864679	38587.401594	31.918938
592.400465	38650.261536	31.923956
592.558264	38724.164776	31.928973
593.096821	38786.664918	31.933991
593.926376	38850.922612	31.939008
594.358754	38924.942289	31.944026
595.040529	38975.094069	31.949044
595.226031	39056.708111	31.954061
595.937431	39116.134987	31.959079
597.105117	39180.896675	31.964096
597.804193	39241.276056	31.969114
598.738035	39309.391000	31.974132
598.884647	39373.416136	31.979149
599.707879	39435.480103	31.984167
600.157453	39521.493657	31.989184
600.682029	39573.746811	31.994202
601.815339	39627.383098	31.999220
602.664651	39687.818059	32.004237
603.217300	39740.363761	32.009255
603.722356	39799.362951	32.014272
604.214086	39874.402535	32.019290
604.615468	39930.250179	32.024308
604.940398	40001.129187	32.029325
605.691956	40055.533682	32.034343
606.280890	40131.880842	32.039360
606.504443	40198.844348	32.044378
607.625751	40277.758829	32.049396
608.006063	40348.292287	32.054413
608.539698	40409.706646	32.059431
608.860727	40479.799014	32.064448
609.612331	40558.128668	32.069466
610.012951	40631.289298	32.074484
610.358899	40720.188643	32.079501
611.201085	40791.651330	32.084519
611.790784	40882.850267	32.089536
612.257822	40962.750149	32.094554
613.183562	41025.541249	32.099572
613.419227	41112.033231	32.104589
613.792838	41187.950010	32.109607
614.606289	41292.116449	32.114624
615.670689	41374.905715	32.119642
616.369362	41449.125234	32.124660
617.023919	41531.717730	32.129677
617.725911	41598.522095	32.134695
618.429104	41681.725958	32.139712
619.252494	41759.367019	32.144730
620.107138	41826.409015	32.149748
620.346971	41904.210201	32.154765
621.187627	41962.576919	32.159783
621.927520	42028.066502	32.164800
622.500381	42102.502002	32.169818
623.208420	42178.557046	32.174836
623.285254	42257.756722	32.179853
624.012925	42326.122140	32.184871
625.060335	42390.653040	32.189888
625.645502	42468.191215	32.194906
626.221244	42534.448424	32.199924
627.153015	42598.134152	32.204941
627.911808	42670.022000	32.209959
628.468130	42734.079584	32.214976
629.030449	42810.625371	32.219994
629.617032	42873.898670	32.225012
629.986333	42949.378279	32.230029
630.711943	43011.647263	32.235047
631.504092	43083.995292	32.240064
632.040801	43156.537327	32.245082
632.681256	43218.416971	32.250100
633.183539	43286.722140	32.255117
633.669224	43343.428099	32.260135
634.428981	43399.204987	32.265152
635.213780	43459.549361	32.270170
636.055312	43514.634319	32.275188
636.418092	43586.117564	32.280205
636.859589	43645.395311	32.285223
637.898082	43709.824948	32.290240
638.090240	43768.828555	32.295258
638.885572	43831.777035	32.300276
639.304794	43904.521355	32.305293
640.017938	43979.992570	32.310311
640.351042	44048.038020	32.315328
640.928976	44121.445242	32.320346
641.711817	44192.476266	32.325364
642.145640	44268.038979	32.330381
642.850289	44349.050854	32.335399
642.943571	44432.595128	32.340416
643.387309	44517.430048	32.345434
644.161203	44593.888254	32.350452
644.679068	44681.149090	32.355469
644.798514	44773.474145	32.360487
645.461840	44871.572975	32.365504
646.265354	44974.438847	32.370522
647.167248	45070.952229	32.375540
648.262117	45163.051810	32.380557
649.295962	45239.914918	32.385575
650.393245	45322.305939	32.390592
651.024357	45414.120246	32.395610
651.509141	45477.551820	32.400628
652.151885	45566.611681	32.405645
653.061579	45638.255585	32.410663
653.441127	45719.557584	32.415680
654.030582	45797.800407	32.420698
654.929224	45875.979864	32.425716
655.285155	45957.435196	32.430733
655.861941	46040.341596	32.435751
656.711569	46109.379639	32.440768
657.571769	46189.574939	32.445786
659.186689	46254.537045	32.450804
659.725196	46325.307081	32.455821
660.562524	46390.161258	32.460839
661.557937	46443.394898	32.465856
662.076685	46516.786556	32.470874
662.862270	46580.948950	32.475892
662.765436	46652.440875	32.480909
663.182588	46713.563785	32.485927
664.187850	46795.370206	32.490944
664.304014	46874.320884	32.495962
664.564164	46954.700641	32.500980
665.022416	47036.503715	32.505997
665.729635	47121.297417	32.511015
666.844601	47210.157607	32.516032
667.076616	47294.815842	32.521050
667.835969	47378.945284	32.526068
668.482952	47467.283998	32.531085
669.068501	47554.891195	32.536103
669.842323	47641.725625	32.541120
670.260871	47747.752239	32.546138
671.027401	47825.187940	32.551156
671.711433	47904.080709	32.556173
672.287864	47998.332375	32.561191
673.412263	48086.238296	32.566208
674.101222	48178.299667	32.571226
675.264817	48250.950513	32.576244
676.150316	48323.341248	32.581261
676.257784	48399.182870	32.586279
677.320120	48479.515564	32.591296
677.785282	48550.271303	32.596314
678.765493	48620.313815	32.601332
679.070395	48680.400540	32.606349
679.475465	48762.456691	32.611367
680.130877	48825.953442	32.616384
680.681885	48917.696955	32.621402
681.318681	48997.738946	32.626420
681.421776	49088.846701	32.631437
681.750875	49176.213186	32.636455
682.649677	49270.383178	32.641472
683.400939	49360.497774	32.646490
684.165998	49449.533611	32.651508
684.647030	49548.545833	32.656525
685.264395	49649.743577	32.661543
686.028746	49745.141357	32.666560
686.327949	49856.884059	32.671578
687.401027	49942.466836	32.676596
688.285495	50029.953945	32.681613
688.952268	50134.958018	32.686631
690.153181	50230.838807	32.691648
690.564177	50330.978332	32.696666
691.099704	50420.662971	32.701684
691.965885	50521.025190	32.706701
692.552030	50607.234572	32.711719
693.708683	50686.938800	32.716736
694.550059	50789.100424	32.721754
695.210752	50884.817873	32.726772
695.681867	50962.466690	32.731789
696.232838	51058.032569	32.736807
697.014334	51158.551070	32.741824
697.726265	51258.175128	32.746842
698.509414	51346.449295	32.751860
699.251992	51441.211625	32.756877
699.732788	51540.338381	32.761895
700.956810	51624.994102	32.766912
701.884636	51706.054253	32.771930
702.828134	51805.099641	32.776948
703.453970	51894.539344	32.781965
704.173561	51975.890853	32.786983
704.838881	52058.748802	32.792000
705.206063	52151.643602	32.797018
706.197050	52227.525002	32.802036
706.829221	52326.251764	32.807053
707.199446	52418.382969	32.812071
708.618847	52493.891443	32.817088
709.021641	52576.327490	32.822106
710.350993	52642.982079	32.827124
711.301560	52717.968715	32.832141
711.783878	52799.824028	32.837159
712.696341	52876.283174	32.842176
713.289283	52963.029442	32.847194
714.042908	53024.859230	32.852212
714.553737	53110.210948	32.857229
715.070508	53191.518927	32.862247
715.930751	53275.828156	32.867264
716.351416	53371.025816	32.872282
716.874948	53458.884993	32.877300
717.764224	53529.917508	32.882317
718.279382	53621.998896	32.887335
718.954773	53709.196052	32.892352
719.580922	53797.147206	32.897370
719.914837	53891.584668	32.902388
720.802271	53985.419450	32.907405
720.811782	54096.236286	32.912423
721.730972	54192.164288	32.917440
722.193225	54299.199009	32.922458
722.933920	54397.153902	32.927476
723.386086	54504.608385	32.932493
724.058947	54602.550236	32.937511
725.338021	54694.099860	32.942528
725.686050	54799.949463	32.947546
726.102564	54905.478749	32.952564
726.968066	55008.457808	32.957581
727.811022	55108.351623	32.962599
728.752617	55202.214881	32.967616
729.410655	55298.191422	32.972634
730.585783	55397.330547	32.977652
731.324183	55494.830078	32.982669
731.762490	55594.066598	32.987687
732.876866	55690.468830	32.992704
733.333029	55786.481090	32.997722
734.086027	55887.145585	33.002740
735.016941	55984.780024	33.007757
735.532245	56082.331939	33.012775
736.417454	56182.394821	33.017792
736.890743	56287.492487	33.022810
737.433654	56386.715718	33.027828
738.162151	56506.627017	33.032845
738.764312	56612.501254	33.037863
739.450379	56726.197174	33.042880
740.135677	56840.904845	33.047898
741.158698	56954.457973	33.052916
742.324720	57055.540425	33.057933
742.980306	57160.922233	33.062951
743.767488	57265.992210	33.067968
744.494509	57369.480357	33.072986
745.043845	57476.442112	33.078004
746.221602	57587.452122	33.083021
746.790628	57704.085939	33.088039
747.445088	57800.650227	33.093056
748.028653	57908.215261	33.098074
748.930780	58022.255736	33.103092
749.487319	58142.634994	33.108109
749.999401	58260.659008	33.113127
750.947529	58382.093512	33.118144
751.442753	58494.807369	33.123162
752.037810	58622.083603	33.128180
752.866116	58744.551156	33.133197
753.567308	58865.656543	33.138215
754.198928	58981.522859	33.143232
754.841603	59110.867048	33.148250
755.908580	59230.094280	33.153268
756.848744	59339.187955	33.158285
758.058115	59461.767588	33.163303
759.313706	59574.779037	33.168320
760.202390	59698.898140	33.173338
760.841833	59796.719475	33.178356
761.472533	59899.155986	33.183373
762.250353	59998.731240	33.188391
763.173792	60101.082522	33.193408
764.037416	60214.111734	33.198426
764.778397	60323.629140	33.203444
766.417046	60413.174020	33.208461
766.997679	60502.590665	33.213479
768.264493	60593.910396	33.218496
769.289358	60670.899323	33.223514
769.630566	60771.586936	33.228532
770.700728	60848.404746	33.233549
770.905107	60947.232519	33.238567
771.672142	61045.152595	33.243584
772.508364	61128.127754	33.248602
772.977131	61227.627386	33.253620
773.788753	61312.863585	33.258637
774.329447	61416.137929	33.263655
775.331684	61511.000456	33.268672
775.714671	61605.504319	33.273690
775.936674	61702.910847	33.278708
777.676157	61779.476304	33.283725
778.846789	61869.522051	33.288743
779.893406	61932.051694	33.293760
780.615549	62013.614636	33.298778
781.230777	62083.964537	33.303796
782.167536	62165.669616	33.308813
782.610408	62253.113215	33.313831
783.421410	62332.968933	33.318848
784.018303	62415.122992	33.323866
784.325246	62499.809156	33.328884
785.017773	62592.370385	33.333901
785.705955	62711.352037	33.338919
786.311389	62814.806080	33.343936
786.887482	62898.425541	33.348954
787.098324	63017.411951	33.353972
788.038121	63126.077334	33.358989
788.407032	63248.199251	33.364007
788.987642	63348.499805	33.369024
790.078151	63493.858675	33.374042
790.853996	63615.207669	33.379060
791.653402	63742.450726	33.384077
792.044508	63865.027741	33.389095
792.724674	63987.090015	33.394112
793.843960	64117.841187	33.399130
793.886007	64246.596688	33.404148
795.034117	64386.952549	33.409165
796.188246	64527.479040	33.414183
796.567290	64656.516464	33.419200
797.088127	64795.449002	33.424218
798.043623	64922.174210	33.429236
799.182585	65053.086092	33.434253
800.465378	65198.659130	33.439271
800.928604	65344.286348	33.444288
801.861031	65482.169424	33.449306
802.656672	65609.772289	33.454324
803.993934	65732.526539	33.459341
804.685208	65862.638800	33.464359
806.028156	65986.563069	33.469376
806.866074	66110.128970	33.474394
807.548041	66247.167162	33.479412
808.127744	66363.355777	33.484429
808.713790	66479.215270	33.489447
809.445157	66601.885059	33.494464
810.416337	66729.762928	33.499482
811.242739	66865.377932	33.504500
812.866864	66985.677332	33.509517
813.359300	67121.184780	33.514535
813.954620	67246.542280	33.519552
815.275364	67356.083647	33.524570
815.365735	67487.152393	33.529588
816.717475	67613.417652	33.534605
817.395547	67741.710460	33.539623
818.045047	67863.870127	33.544640
818.966500	67993.590986	33.549658
819.869965	68121.140829	33.554676
820.641675	68252.038624	33.559693
821.064391	68381.243630	33.564711
821.632322	68515.034314	33.569728
822.582904	68651.847904	33.574746
823.197617	68781.156425	33.579764
823.895081	68917.552010	33.584781
824.942818	69063.323566	33.589799
825.208597	69193.564712	33.594816
826.579905	69331.432298	33.599834
827.337840	69461.979498	33.604852
828.645837	69596.773909	33.609869
830.144441	69712.519520	33.614887
830.693100	69828.372040	33.619904
831.834329	69935.433772	33.624922
832.724249	70041.070690	33.629940
833.670183	70153.198583	33.634957
834.625628	70250.764331	33.639975
835.586826	70355.942136	33.644992
836.613344	70447.914090	33.650010
837.108623	70564.367455	33.655028
838.230838	70664.152153	33.660045
838.875490	70780.841272	33.665063
839.381373	70888.278273	33.670080
840.620619	70978.763134	33.675098
841.476008	71095.039801	33.680116
842.072672	71204.461454	33.685133
843.606325	71294.020148	33.690151
844.074824	71402.926526	33.695168
845.020394	71497.154729	33.700186
846.242224	71591.375671	33.705204
847.203583	71687.461096	33.710221
847.989968	71802.905711	33.715239
848.316947	71906.254673	33.720256
849.202450	72001.291736	33.725274
849.629459	72118.529949	33.730292
850.515226	72233.498874	33.735309
851.352447	72350.828703	33.740327
852.342603	72478.055256	33.745344
852.977511	72600.162364	33.750362
853.504527	72733.259121	33.755380
854.203673	72844.449101	33.760397
854.798478	72966.368879	33.765415
855.439709	73104.514187	33.770432
856.533697	73237.191611	33.775450
857.466054	73375.720587	33.780468
858.126825	73506.201018	33.785485
858.663933	73639.719055	33.790503
859.400618	73784.157664	33.795520
860.812510	73925.652696	33.800538
861.219503	74078.874515	33.805556
862.266050	74217.731508	33.810573
862.992518	74354.156946	33.815591
863.573387	74508.289020	33.820608
864.533498	74652.841966	33.825626
865.240374	74793.687537	33.830644
866.557184	74946.992910	33.835661
867.401381	75089.259605	33.840679
868.328380	75235.213186	33.845696
869.398077	75382.598746	33.850714
870.050421	75534.734148	33.855732
870.743061	75673.507070	33.860749
871.689753	75811.739301	33.865767
872.891850	75950.429859	33.870784
874.081509	76080.294487	33.875802
874.830034	76239.242926	33.880820
876.254647	76372.087247	33.885837
877.281926	76504.934733	33.890855
877.789156	76639.348835	33.895872
878.998993	76756.944492	33.900890
879.663564	76899.904030	33.905908
880.848866	77036.611958	33.910925
882.165195	77143.806989	33.915943
883.179563	77262.670938	33.920960
884.856531	77377.846304	33.925978
885.409318	77498.969784	33.930996
886.220434	77621.107523	33.936013
887.276383	77735.425916	33.941031
887.608802	77848.125015	33.946048
888.396239	77953.184934	33.951066
889.277349	78090.449277	33.956084
889.841171	78196.799616	33.961101
890.583383	78308.623791	33.966119
891.296814	78423.248961	33.971136
891.932974	78538.602217	33.976154
892.580845	78671.588617	33.981172
892.928859	78790.128021	33.986189
894.332250	78921.776737	33.991207
895.006427	79064.856178	33.996224
895.880258	79187.283132	34.001242
896.556499	79328.687722	34.006260
897.234612	79473.021542	34.011277
898.402689	79610.273171	34.016295
898.914779	79757.128444	34.021312
899.945913	79895.258367	34.026330
900.871930	80041.737213	34.031348
901.870217	80181.158402	34.036365
902.957687	80323.114951	34.041383
904.317009	80456.374031	34.046400
905.996631	80584.526800	34.051418
906.912203	80710.073742	34.056436
907.761204	80850.700317	34.061453
908.919174	80968.655731	34.066471
909.514851	81107.851827	34.071488
910.594255	81232.501667	34.076506
911.476377	81362.194877	34.081524
912.049671	81498.025370	34.086541
913.019076	81628.180140	34.091559
913.876306	81761.517184	34.096576
915.957812	81860.365735	34.101594
917.195027	81971.038360	34.106612
918.052575	82092.882842	34.111629
919.153994	82215.642960	34.116647
919.526082	82335.911452	34.121664
920.534393	82434.724615	34.126682
921.148384	82565.455868	34.131700
922.023116	82680.828931	34.136717
922.891569	82810.045556	34.141735
923.116112	82968.672833	34.146752
924.201123	83097.463098	34.151770
925.352528	83229.077362	34.156788
926.078222	83363.641209	34.161805
926.917263	83491.354524	34.166823
927.181269	83650.713889	34.171840
927.895831	83799.757248	34.176858
928.846389	83959.587451	34.181876
929.387380	84104.289752	34.186893
930.616790	84255.610911	34.191911
931.351189	84423.451673	34.196928
932.104543	84574.265140	34.201946
932.967150	84751.653230	34.206964
933.306708	84915.026422	34.211981
934.478011	85082.559427	34.216999
935.261989	85251.195220	34.222016
936.301711	85413.842622	34.227034
937.155917	85597.116389	34.232052
937.852525	85755.830464	34.237069
939.310441	85929.896152	34.242087
939.701814	86118.210943	34.247104
940.785871	86292.018383	34.252122
941.908372	86462.505268	34.257140
942.994542	86650.747619	34.262157
943.817251	86816.167762	34.267175
944.817888	87001.465843	34.272192
945.746191	87179.019825	34.277210
946.744367	87346.774911	34.282228
948.004239	87517.006373	34.287245
948.966396	87686.845291	34.292263
949.522704	87868.983852	34.297280
950.317908	88028.905695	34.302298
951.532874	88201.902101	34.307316
952.348361	88359.608125	34.312333
953.094664	88522.078848	34.317351
954.304295	88683.018778	34.322368
955.343651	88854.277158	34.327386
956.605787	89008.863712	34.332404
957.509726	89189.505976	34.337421
958.698425	89341.708507	34.342439
959.208828	89507.161178	34.347456
960.045049	89675.149431	34.352474
961.155350	89850.098952	34.357492
962.405738	90030.728396	34.362509
963.344172	90193.267462	34.367527
963.785900	90363.527960	34.372544
965.207551	90530.647216	34.377562
966.152548	90696.080704	34.382580
967.182725	90881.537254	34.387597
968.648601	91036.780517	34.392615
969.332699	91207.646198	34.397632
970.436136	91376.931326	34.402650
971.764155	91544.781937	34.407668
972.330957	91701.241158	34.412685
973.590103	91856.897260	34.417703
974.435722	92028.710418	34.422720
975.741455	92198.676765	34.427738
976.876159	92367.900425	34.432756
977.559209	92534.972059	34.437773
978.943495	92682.682703	34.442791
980.337058	92843.417801	34.447808
981.797813	92988.839252	34.452826
982.895294	93134.783576	34.457844
983.933952	93292.839765	34.462861
985.284157	93440.389778	34.467879
985.743917	93592.410538	34.472896
986.398063	93742.969750	34.477914
987.622592	93882.555703	34.482932
988.637028	94048.215934	34.487949
989.852547	94200.039766	34.492967
990.274855	94356.464053	34.497984
990.778632	94515.167147	34.503002
991.937901	94667.528517	34.508020
992.585654	94833.583748	34.513037
993.676061	94995.655356	34.518055
994.325296	95171.808287	34.523072
995.046582	95353.147231	34.528090
996.180804	95529.577119	34.533108
997.186958	95707.238399	34.538125
997.901224	95872.011062	34.543143
999.045601	96068.002182	34.548160
999.757811	96248.716236	34.553178
1000.948971	96427.820697	34.558196
1001.721602	96624.308039	34.563213
1002.975730	96798.840876	34.568231
1004.252952	96968.667891	34.573248
1005.690208	97153.896132	34.578266
1006.384654	97330.987529	34.583284
1007.218607	97503.480417	34.588301
1008.372389	97677.327014	34.593319
1009.669255	97857.183971	34.598336
1010.544737	98041.099906	34.603354
1011.615121	98217.217636	34.608372
1012.532148	98396.027035	34.613389
1013.954752	98572.184072	34.618407
1015.379808	98743.847277	34.623424
1016.380345	98908.282607	34.628442
1017.379940	99067.907914	34.633460
1018.233964	99234.756205	34.638477
1019.552202	99383.163661	34.643495
1020.507492	99536.911729	34.648512
1021.031954	99687.515837	34.653530
1022.097092	99849.756212	34.658548
1022.795558	100014.957686	34.663565
1023.648140	100175.070095	34.668583
1024.717838	100336.356877	34.673600
1025.473000	100507.458951	34.678618
1026.341931	100663.488278	34.683636
1027.694804	100846.668475	34.688653
1028.302119	101013.543905	34.693671
1029.430128	101197.542476	34.698688
1030.458319	101385.262593	34.703706
1031.784759	101546.558988	34.708724
1032.280192	101726.955716	34.713741
1033.351217	101893.538754	34.718759
1034.719089	102097.985990	34.723776
1035.533769	102271.742913	34.728794
1036.961847	102443.468660	34.733812
1038.459227	102616.260467	34.738829
1040.301819	102777.371772	34.743847
1041.487092	102948.438181	34.748864
1042.482968	103110.438478	34.753882
1043.723586	103277.135458	34.758900
1044.517203	103446.838879	34.763917
1045.789126	103604.256886	34.768935
1046.897231	103762.709646	34.773952
1047.663093	103921.625110	34.778970
1049.098333	104074.985662	34.783988
1050.299794	104239.897068	34.789005
1051.382972	104393.551902	34.794023
1052.154178	104549.855248	34.799040
1053.077169	104724.351623	34.804058
1054.189314	104894.227212	34.809076
1054.888437	105052.590720	34.814093
1055.947987	105220.469847	34.819111
1056.837519	105390.746346	34.824128
1057.563491	105585.670555	34.829146
1058.194192	105748.558100	34.834164
1058.755263	105935.558833	34.839181
1060.068106	106140.192663	34.844199
1060.819606	106330.432254	34.849216
1061.279515	106541.593052	34.854234
1062.577979	106745.537390	34.859252
1063.128848	106947.225686	34.864269
1064.461230	107152.839355	34.869287
1065.771046	107362.219930	34.874304
1067.149441	107577.302916	34.879322
1068.086470	107771.055874	34.884340
1068.865626	107972.815603	34.889357
1069.658460	108184.301823	34.894375
1071.199716	108394.146277	34.899392
1072.257453	108607.099340	34.904410
1073.721989	108806.485040	34.909428
1074.654323	109013.027734	34.914445
1075.654207	109226.349922	34.919463
1077.064159	109428.054494	34.924480
1078.098223	109621.500850	34.929498
1079.384615	109828.105359	34.934516
1080.410323	110040.809085	34.939533
1081.474981	110244.502084	34.944551
1082.332900	110449.142751	34.949568
1083.188802	110662.297398	34.954586
1084.515739	110862.823047	34.959604
1085.289389	111071.789074	34.964621
1086.113874	111286.904528	34.969639
1086.936129	111513.739222	34.974656
1087.692046	111734.531773	34.979674
1088.972770	111937.999119	34.984692
1090.266258	112152.271258	34.989709
1091.686102	112356.833494	34.994727
1093.133060	112545.976193	34.999744
1094.185576	112754.110981	35.004762
1095.582603	112941.060448	35.009780
1097.119760	113134.778081	35.014797
1098.264518	113320.504972	35.019815
1099.464606	113507.668146	35.024832
1100.187853	113713.964314	35.029850
1101.219294	113892.733561	35.034868
1102.199018	114099.230956	35.039885
1103.329223	114294.569437	35.044903
1105.119818	114469.809259	35.049920
1106.196584	114677.397097	35.054938
1107.307000	114862.379862	35.059956
1108.435571	115054.164023	35.064973
1109.124573	115256.968016	35.069991
1110.461442	115449.860710	35.075008
1111.124651	115647.046741	35.080026
1112.351911	115838.718631	35.085044
1113.280504	116052.447680	35.090061
1114.226871	116270.989783	35.095079
1115.644548	116463.964785	35.100096
1116.496321	116681.930223	35.105114
1117.580967	116897.426322	35.110132
1118.778288	117112.107267	35.115149
1119.900299	117322.785923	35.120167
1120.982604	117521.993723	35.125184
1121.724644	117748.398317	35.130202
1123.163871	117963.970679	35.135220
1124.146172	118190.199748	35.140237
1125.508305	118415.468314	35.145255
1126.952918	118617.487455	35.150272
1127.792551	118832.557163	35.155290
1129.131878	119037.295465	35.160308
1130.425223	119261.150250	35.165325
1131.689366	119489.357687	35.170343
1133.190313	119705.414445	35.175360
1133.898175	119918.309276	35.180378
1135.195455	120128.574156	35.185396
1136.089216	120344.900645	35.190413
1136.991728	120565.370813	35.195431
1138.370628	120771.191928	35.200448
1139.434010	121007.541474	35.205466
1140.783890	121226.270164	35.210484
1141.786932	121435.452622	35.215501
1142.906887	121648.963689	35.220519
1144.581547	121873.307884	35.225536
1145.608037	122097.177879	35.230554
1146.836663	122297.408198	35.235572
1147.897994	122514.762195	35.240589
1148.726818	122748.731447	35.245607
1150.133602	122951.268489	35.250624
1150.919950	123175.794586	35.255642
1152.327880	123393.541367	35.260660
1153.685724	123623.552421	35.265677
1154.669239	123838.014279	35.270695
1155.820765	124056.669988	35.275712
1157.056875	124266.454995	35.280730
1158.667145	124472.377824	35.285748
1159.952856	124691.535624	35.290765
1160.914171	124911.483618	35.295783
1162.708026	125092.135501	35.300800
1164.413716	125306.121158	35.305818
1165.499093	125503.595899	35.310836
1166.527076	125704.275126	35.315853
1167.520163	125895.152107	35.320871
1168.626350	126086.062318	35.325888
1169.395710	126275.166295	35.330906
1170.369878	126457.862722	35.335924
1171.841497	126647.778290	35.340941
1172.752788	126849.130731	35.345959
1173.518910	127040.610037	35.350976
1173.985031	127253.027025	35.355994
1175.183186	127464.843034	35.361012
1176.325427	127682.347830	35.366029
1177.139564	127893.621827	35.371047
1178.336452	128113.490772	35.376064
1179.705843	128339.771501	35.381082
1180.620493	128554.151392	35.386100
1181.728067	128791.860509	35.391117
1182.363227	129032.970248	35.396135
1183.481839	129265.763338	35.401152
1184.362158	129513.199174	35.406170
1185.322864	129776.100084	35.411188
1186.246420	130027.234018	35.416205
1187.215591	130289.516770	35.421223
1188.730213	130533.357598	35.426240
1189.645942	130810.978192	35.431258
1191.017564	131090.009045	35.436276
1192.611858	131336.504858	35.441293
1194.099839	131597.546729	35.446311
1195.292697	131844.911359	35.451328
1196.628629	132104.017729	35.456346
1198.010145	132355.893255	35.461364
1199.891547	132606.876982	35.466381
1201.332107	132856.895991	35.471399
1203.004805	133080.105878	35.476416
1204.659724	133315.768667	35.481434
1205.928922	133550.875701	35.486452
1207.211154	133778.439629	35.491469
1208.442183	134008.548992	35.496487
1210.046813	134238.712426	35.501504
1210.885746	134468.534839	35.506522
1212.027668	134691.856216	35.511540
1213.564557	134910.372663	35.516557
1214.660091	135144.353677	35.521575
1216.188480	135386.936269	35.526592
1217.156507	135611.585772	35.531610
1217.916135	135836.220510	35.536628
1219.427085	136057.969050	35.541645
1220.306781	136299.892163	35.546663
1221.593645	136535.550387	35.551680
1222.762516	136780.801620	35.556698
1223.647523	137014.551847	35.561716
1225.026544	137251.201548	35.566733
1226.316333	137489.870829	35.571751
1227.624800	137740.595814	35.576768
1228.324023	137995.657840	35.581786
1229.597908	138242.753621	35.586804
1230.879561	138477.133329	35.591821
1231.754777	138733.579275	35.596839
1232.838223	138981.523392	35.601856
1234.118383	139241.950921	35.606874
1235.081814	139494.609821	35.611892
1236.555449	139764.429938	35.616909
1237.753218	140029.365547	35.621927
1238.919592	140273.958191	35.626944
1240.220104	140537.879159	35.631962
1241.323503	140792.426555	35.636980
1242.906837	141060.146772	35.641997
1244.214623	141314.867208	35.647015
1245.079837	141573.048082	35.652032
1246.350517	141844.401733	35.657050
1247.635643	142106.638264	35.662068
1248.978466	142350.848939	35.667085
1249.911473	142606.376255	35.672103
1251.390461	142838.648590	35.677120
1252.525358	143086.271717	35.682138
1253.428729	143347.439443	35.687156
1254.814693	143599.678494	35.692173
1255.717153	143865.618120	35.697191
1257.165181	144116.176823	35.702208
1258.323264	144375.585627	35.707226
1259.869887	144628.312810	35.712244
1261.487237	144885.557235	35.717261
1262.318436	145145.076391	35.722279
1263.562537	145412.505738	35.727296
1265.056132	145685.665889	35.732314
1266.192952	145936.162079	35.737332
1267.477876	146199.304327	35.742349
1268.697171	146462.116947	35.747367
1269.961889	146742.513398	35.752384
1271.561685	147018.747863	35.757402
1271.973304	147289.930291	35.762420
1273.797852	147563.138935	35.767437
1274.736289	147842.951038	35.772455
1276.077185	148113.098529	35.777472
1277.347411	148408.116798	35.782490
1278.433106	148697.004318	35.787508
1279.693701	148970.468828	35.792525
1281.055402	149257.780659	35.797543
1282.126237	149537.621972	35.802560
1283.700228	149835.277645	35.807578
1284.645227	150127.636667	35.812596
1286.305563	150428.161867	35.817613
1287.810480	150719.837058	35.822631
1288.811558	151009.986943	35.827648
1290.297140	151291.929195	35.832666
1291.610447	151592.394246	35.837684
1293.147488	151876.399788	35.842701
1294.611207	152175.411462	35.847719
1296.362169	152453.450185	35.852736
1297.944423	152735.057548	35.857754
1299.109618	153014.541547	35.862772
1300.944650	153270.946580	35.867789
1302.515868	153543.759172	35.872807
1304.334479	153809.061989	35.877824
1307.301135	154022.971399	35.882842
1309.028389	154264.306817	35.887860
1310.647673	154484.237855	35.892877
1311.795206	154722.843244	35.897895
1312.749044	154958.704189	35.902912
1314.008374	155185.611643	35.907930
1314.953966	155422.998918	35.912948
1315.831360	155651.874819	35.917965
1316.966968	155903.237511	35.922983
1317.950885	156153.358377	35.928000
1319.426942	156405.340407	35.933018
1319.950086	156664.927403	35.938036
1321.099228	156918.463507	35.943053
1321.962541	157185.748362	35.948071
1323.126244	157439.716707	35.953088
1324.539411	157714.208384	35.958106
1325.600759	157992.337306	35.963124
1326.751937	158263.083079	35.968141
1328.051080	158533.857010	35.973159
1329.605436	158821.437201	35.978176
1331.077024	159088.000150	35.983194
1331.987072	159355.190345	35.988212
1333.720207	159629.312519	35.993229
1334.876722	159912.538775	35.998247
1336.230666	160190.355523	36.003264
1337.349249	160465.764580	36.008282
1338.184337	160725.339092	36.013300
1339.892744	160994.108260	36.018317
1340.872359	161260.474873	36.023335
1342.233881	161538.134599	36.028352
1343.840803	161807.458665	36.033370
1344.571293	162101.427095	36.038388
1345.947183	162377.275887	36.043405
1346.974984	162661.950567	36.048423
1348.789170	162939.786017	36.053440
1350.229196	163228.151853	36.058458
1351.773848	163507.532620	36.063476
1353.452322	163782.414580	36.068493
1354.785990	164067.872983	36.073511
1355.839697	164353.125767	36.078528
1356.998806	164638.807131	36.083546
1358.019844	164949.507631	36.088564
1359.095049	165238.023486	36.093581
1360.463298	165543.646698	36.098599
1361.812859	165858.423071	36.103616
1363.050550	166157.474528	36.108634
1364.280694	166475.282131	36.113652
1365.875645	166774.443826	36.118669
1367.357641	167086.415881	36.123687
1368.949728	167409.474214	36.128704
1370.415296	167721.263179	36.133722
1371.476438	168039.186167	36.138740
1373.019605	168353.923203	36.143757
1374.307441	168666.331842	36.148775
1375.793355	168982.135934	36.153792
1377.393934	169290.310063	36.158810
1378.604340	169621.365313	36.163828
1379.823944	169947.333202	36.168845
1381.124552	170272.757137	36.173863
1382.387629	170607.465380	36.178880
1383.830936	170937.628969	36.183898
1384.888808	171264.204025	36.188916
1386.598552	171591.930084	36.193933
1388.239535	171922.080839	36.198951
1389.544405	172247.353166	36.203968
1391.151827	172570.928185	36.208986
1392.503878	172910.333705	36.214004
1394.500342	173233.024286	36.219021
1395.840788	173557.068972	36.224039
1397.452364	173882.568574	36.229056
1398.692847	174191.291843	36.234074
1399.662032	174528.069229	36.239092
1401.159672	174857.033384	36.244109
1402.445039	175186.275956	36.249127
1403.938314	175507.770659	36.254144
1406.707662	175815.769894	36.259162
1408.417322	176120.582953	36.264180
1410.005196	176425.532246	36.269197
1411.475689	176727.951969	36.274215
1412.669496	177040.470414	36.279232
1414.773626	177339.197830	36.284250
1415.861445	177645.506354	36.289268
1417.057872	177935.808039	36.294285
1418.591301	178245.917538	36.299303
1419.592965	178542.943180	36.304320
1421.371904	178845.718416	36.309338
1422.586597	179145.111147	36.314356
1424.050507	179436.671951	36.319373
1425.180530	179758.241669	36.324391
1426.194889	180067.826203	36.329408
1427.966332	180382.085160	36.334426
1429.003130	180695.845390	36.339444
1430.433502	181003.475865	36.344461
1432.222798	181292.772517	36.349479
1433.365833	181585.820055	36.354496
1435.165321	181866.716110	36.359514
1436.378359	182168.804858	36.364532
1437.996834	182466.576543	36.369549
1439.271167	182766.412098	36.374567
1440.393206	183048.479760	36.379584
1441.689588	183339.112952	36.384602
1443.525779	183649.839783	36.389620
1445.037909	183940.948367	36.394637
1446.682460	184243.688561	36.399655
1447.613218	184565.676228	36.404672
1449.142481	184863.336451	36.409690
1450.403247	185171.920429	36.414708
1451.086652	185491.923563	36.419725
1452.589384	185807.033477	36.424743
1453.624132	186133.189282	36.429760
1455.445171	186461.730518	36.434778
1456.682161	186799.521935	36.439796
1457.893918	187154.201724	36.444813
1459.370207	187487.083578	36.449831
1460.468691	187833.446787	36.454848
1461.756466	188181.824555	36.459866
1463.174522	188552.968093	36.464884
1464.704524	188908.964634	36.469901
1466.639441	189262.116627	36.474919
1467.619374	189624.834563	36.479936
1469.531133	189961.733782	36.484954
1470.703832	190330.314332	36.489972
1472.722698	190680.731907	36.494989
1474.191640	191039.125429	36.500007
1475.799528	191396.736545	36.505024
1477.558139	191761.509958	36.510042
1479.218331	192105.635299	36.515060
1480.771846	192458.488657	36.520077
1482.190931	192815.365063	36.525095
1483.382279	193178.273035	36.530112
1485.076805	193534.181507	36.535130
1486.216650	193903.995539	36.540148
1487.198214	194268.328331	36.545165
1488.805542	194629.995627	36.550183
1490.299900	195008.466508	36.555200
1492.316065	195372.482705	36.560218
1493.901514	195742.729250	36.565236
1495.541265	196108.246366	36.570253
1497.035576	196460.230967	36.575271
1498.562359	196837.831471	36.580288
1500.074715	197205.584880	36.585306
1501.994790	197563.332486	36.590324
1503.562963	197912.126239	36.595341
1505.257737	198260.647048	36.600359
1506.681239	198620.462902	36.605376
1508.748623	198973.991598	36.610394
1510.355554	199335.596563	36.615412
1511.604341	199684.731669	36.620429
1513.349096	200025.077276	36.625447
1514.452668	200388.929278	36.630464
1515.956359	200737.583384	36.635482
1517.243035	201107.604718	36.640500
1518.251501	201471.313105	36.645517
1519.735701	201826.666874	36.650535
1520.801522	202207.268483	36.655552
1522.718012	202578.234811	36.660570
1523.897299	202960.142193	36.665588
1525.436563	203352.517724	36.670605
1526.954622	203716.509100	36.675623
1528.065572	204107.207279	36.680640
1529.622501	204458.308763	36.685658
1531.244857	204834.083872	36.690676
1532.781142	205203.945627	36.695693
1534.474287	205567.777659	36.700711
1535.492858	205929.805518	36.705728
1536.598857	206289.268571	36.710746
1537.980588	206675.682065	36.715764
1539.336955	207076.322636	36.720781
1540.852302	207461.295959	36.725799
1541.838000	207862.204936	36.730816
1543.965258	208225.089204	36.735834
1546.120719	208622.672793	36.740852
1547.303632	209000.699525	36.745869
1549.448307	209390.314667	36.750887
1551.240615	209780.281892	36.755904
1553.114125	210158.428684	36.760922
1554.914125	210533.275233	36.765940
1556.726500	210933.809250	36.770957
1558.141739	211296.812153	36.775975
1559.957082	211669.528068	36.780992
1561.808646	212050.163239	36.786010
1563.370885	212424.905150	36.791028
1564.635456	212810.161105	36.796045
1566.231698	213185.230883	36.801063
1567.424750	213566.616358	36.806080
1568.855796	213949.843579	36.811098
1570.304138	214351.253692	36.816116
1571.593186	214751.726819	36.821133
1573.126000	215152.821833	36.826151
1574.459068	215550.497577	36.831168
1576.128057	215966.100852	36.836186
1577.468754	216369.061505	36.841204
1579.233292	216775.661995	36.846221
1580.992962	217194.455871	36.851239
1582.467612	217618.098785	36.856256
1584.045340	218005.026788	36.861274
1585.570745	218411.419741	36.866292
1587.291790	218913.176947	36.871309
1589.291430	219321.324074	36.876327
1590.376835	219734.677964	36.881344
1592.429120	220134.387511	36.886362
1593.780473	220558.393569	36.891380
1595.214808	220990.286622	36.896397
1597.086137	221415.454926	36.901415
1598.954652	221827.722862	36.906432
1600.648252	222238.776717	36.911450
1602.360438	222637.256616	36.916468
1603.995222	223062.851491	36.921485
1605.074141	223478.430887	36.926503
1606.877707	223911.417724	36.931520
1608.329982	224332.628117	36.936538
1610.290352	224741.615327	36.941556
1611.158532	225169.046428	36.946573
1613.132379	225591.521546	36.951591
1615.342807	226038.292030	36.956608
1616.996465	226440.477869	36.961626
1618.980660	226853.227645	36.966644
1620.498095	227278.577994	36.971661
1622.440882	227683.717410	36.976679
1624.299108	228089.913492	36.981696
1626.035799	228489.425280	36.986714
1627.734699	228901.568471	36.991732
1628.854852	229307.966379	36.996749
1630.671552	229712.650387	37.001767
1631.835356	230139.262364	37.006784
1633.854946	230536.981040	37.011802
1635.225055	230953.528300	37.016820
1636.986481	231375.193986	37.021837
1638.316753	231768.330776	37.026855
1640.092889	232170.183777	37.031872
1641.639321	232554.218936	37.036890
1643.140768	232957.694277	37.041908
1644.429730	233361.332769	37.046925
1646.103738	233752.284445	37.051943
1648.280899	234152.603341	37.056960
1649.638139	234553.820577	37.061978
1651.588026	234946.457006	37.066996
1653.299524	235360.064461	37.072013
1654.790114	235757.452481	37.077031
1656.416358	236147.909856	37.082048
1658.008794	236559.990441	37.087066
1659.435504	236964.301055	37.092084
1661.062962	237376.809626	37.097101
1662.356365	237798.112463	37.102119
1663.656114	238224.698804	37.107136
1664.856551	238653.969707	37.112154
1666.932778	239078.956578	37.117172
1668.387762	239516.976486	37.122189
1670.448197	239964.321631	37.127207
1671.800970	240399.439111	37.132224
1673.491121	240851.292662	37.137242
1674.516766	241275.924057	37.142260
1676.121907	241738.614850	37.147277
1678.430540	242200.022042	37.152295
1679.955892	242654.954794	37.157312
1681.824209	243111.355998	37.162330
1683.862363	243565.062800	37.167348
1685.583856	244027.611949	37.172365
1687.471101	244471.819372	37.177383
1689.415945	244925.112178	37.182400
1690.710703	245374.397784	37.187418
1692.482256	245824.011905	37.192436
1693.720686	246283.647153	37.197453
1696.048612	246736.219232	37.202471
1698.188496	247195.453139	37.207488
1699.909985	247644.697232	37.212506
1701.852058	248094.134183	37.217524
1703.762910	248545.710728	37.222541
1705.619831	248979.336894	37.227559
1707.426978	249440.152942	37.232576
1709.015347	249882.207445	37.237594
1710.773776	250325.123492	37.242612
1712.496232	250772.745512	37.247629
1714.306394	251219.642241	37.252647
1715.586641	251663.705483	37.257664
1717.710548	252123.557700	37.262682
1719.804706	252571.577389	37.267700
1721.073669	253019.225531	37.272717
1722.734062	253461.068336	37.277735
1724.493726	253906.349921	37.282752
1726.091881	254362.810464	37.287770
1728.050504	254817.789259	37.292788
1729.290017	255271.286562	37.297805
1731.634303	255721.096207	37.302823
1733.561696	256166.351461	37.307840
1735.094947	256611.900568	37.312858
1737.148797	257058.761145	37.317876
1738.901782	257507.830793	37.322893
1740.798815	257945.013475	37.327911
1743.098312	258391.910138	37.332928
1744.373479	258827.595202	37.337946
1746.527559	259255.158695	37.342964
1747.887497	259709.958576	37.347981
1749.904406	260144.022615	37.352999
1751.346951	260582.601589	37.358016
1752.607674	261023.700068	37.363034
1754.048712	261463.422388	37.368052
1756.353530	261897.159391	37.373069
1758.081193	262306.020094	37.378087
1760.066384	262729.267297	37.383104
1761.625283	263135.335888	37.388122
1763.652261	263547.068284	37.393140
1765.223818	263976.429331	37.398157
1767.568769	264371.342825	37.403175
1769.906585	264783.861787	37.408192
1771.453706	265197.806568	37.413210
1773.304174	265607.280937	37.418228
1774.827315	266025.751014	37.423245
1776.462699	266433.583794	37.428263
1778.621568	266839.069081	37.433280
1780.096374	267251.957658	37.438298
1782.411566	267657.721443	37.443316
1784.003571	268075.645311	37.448333
1785.274519	268484.933949	37.453351
1787.427185	268902.612228	37.458368
1788.489550	269345.898457	37.463386
1790.167176	269764.263994	37.468404
1791.770628	270203.395613	37.473421
1792.467922	270655.707972	37.478439
1794.441092	271113.550398	37.483456
1795.836215	271587.135818	37.488474
1797.344352	272043.885268	37.493492
1799.121244	272532.775181	37.498509
1801.214216	273015.337741	37.503527
1802.854175	273493.655834	37.508544
1804.522168	273969.148860	37.513562
1806.614303	274439.363608	37.518580
1808.199993	274935.978268	37.523597
1809.710136	275418.861701	37.528615
1811.767537	275905.261153	37.533632
1813.996146	276406.949161	37.538650
1815.815418	276897.831453	37.543668
1817.299453	277403.806282	37.548685
1819.179378	277898.410688	37.553703
1821.482640	278403.232129	37.558720
1822.679663	278914.941111	37.563738
1824.915324	279408.924666	37.568756
1826.287570	279913.362761	37.573773
1828.210461	280414.990779	37.578791
1830.304155	280940.162415	37.583808
1831.972838	281455.623029	37.588826
1833.909429	281958.565766	37.593844
1835.645313	282481.556864	37.598861
1837.562917	282994.609835	37.603879
1839.183962	283521.681155	37.608896
1841.043985	284037.966616	37.613914
1842.893057	284555.446200	37.618932
1844.811748	285088.026535	37.623949
1846.137179	285622.455699	37.628967
1848.152260	286157.480561	37.633984
1850.092730	286698.408978	37.639002
1851.432537	287222.466686	37.644020
1853.319137	287773.433600	37.649037
1855.128855	288325.046173	37.654055
1857.171787	288868.134329	37.659072
1859.204498	289409.012248	37.664090
1861.254012	289924.764143	37.669108
1863.474217	290461.009532	37.674125
1865.742128	290986.144963	37.679143
1867.956261	291511.388791	37.684160
1869.606177	292038.425388	37.689178
1872.116263	292548.706292	37.694196
1874.170488	293078.161105	37.699213
1875.967182	293587.082264	37.704231
1878.293400	294092.408797	37.709248
1879.845502	294590.647408	37.714266
1881.687591	295067.144893	37.719284
1883.602749	295537.049935	37.724301
1885.724659	296017.383490	37.729319
1887.539003	296496.622792	37.734336
1889.285185	296979.223983	37.739354
1891.537003	297446.398674	37.744372
1893.466261	297932.800752	37.749389
1895.151918	298413.729292	37.754407
1897.374659	298879.327878	37.759424
1899.173216	299366.506959	37.764442
1901.128227	299848.171898	37.769460
1902.904164	300330.778464	37.774477
1904.703867	300822.877748	37.779495
1907.382598	301285.520259	37.784512
1909.481069	301761.387072	37.789530
1911.532898	302234.846484	37.794548
1913.302016	302698.572105	37.799565
1915.505240	303173.195643	37.804583
1917.385880	303660.365568	37.809600
1918.834071	304147.807480	37.814618
1920.607515	304625.643846	37.819636
1922.825260	305102.871108	37.824653
1924.180742	305606.371522	37.829671
1926.015116	306079.187015	37.834688
1928.226396	306589.753425	37.839706
1930.185016	307084.485747	37.844724
1931.853384	307590.208960	37.849741
1932.874267	308090.753600	37.854759
1935.123477	308599.092453	37.859776
1936.980943	309123.898604	37.864794
1938.458256	309643.964370	37.869812
1940.411981	310176.925415	37.874829
1942.193966	310698.813527	37.879847
1944.427113	311226.769503	37.884864
1946.257356	311763.778307	37.889882
1948.200751	312300.561649	37.894900
1950.268662	312837.168411	37.899917
1952.719463	313353.824385	37.904935
1955.175851	313871.263189	37.909952
1957.645642	314405.761164	37.914970
1959.566644	314922.798602	37.919988
1961.710233	315449.242254	37.925005
1963.328396	315971.274145	37.930023
1965.075543	316499.883345	37.935040
1966.741074	317031.650923	37.940058
1969.420637	317543.009014	37.945076
1971.109501	318067.426440	37.950093
1973.054457	318607.084152	37.955111
1975.143580	319121.778458	37.960128
1976.593434	319663.185554	37.965146
1978.856898	320208.288402	37.970164
1980.908240	320745.753508	37.975181
1982.246412	321284.677721	37.980199
1984.118903	321819.853084	37.985216
1985.905517	322373.015342	37.990234
1987.780208	322920.953240	37.995252
1990.030589	323474.359776	38.000269
1992.429932	324029.336609	38.005287
1994.901781	324562.156200	38.010304
1996.509230	325103.187979	38.015322
1998.179881	325650.679137	38.020340
2000.027223	326218.016550	38.025357
2001.681856	326777.738290	38.030375
2003.884025	327330.179439	38.035392
2005.971189	327891.342994	38.040410
2007.541658	328449.590666	38.045428
2009.288723	329013.135611	38.050445
2011.436587	329565.615936	38.055463
2013.951177	330082.055595	38.060480
2015.788781	330633.739219	38.065498
2017.348167	331170.941733	38.070516
2019.509172	331713.599853	38.075533
2021.147095	332277.562773	38.080551
2023.494112	332818.250247	38.085568
2025.758667	333347.014372	38.090586
2028.269411	333896.092817	38.095604
2030.453628	334427.804740	38.100621
2032.150674	334982.439225	38.105639
2034.190970	335519.825351	38.110656
2036.325721	336077.498919	38.115674
2038.449958	336633.137626	38.120692
2040.484941	337187.947569	38.125709
2042.127550	337742.232572	38.130727
2043.901807	338308.852214	38.135744
2045.868748	338875.510085	38.140762
2047.764083	339441.310526	38.145780
2049.788446	340023.354311	38.150797
2051.336325	340610.140570	38.155815
2053.246145	341189.347002	38.160832
2054.979563	341787.282877	38.165850
2057.076542	342400.761776	38.170868
2058.925565	343012.674921	38.175885
2060.781019	343632.422350	38.180903
2063.148456	344253.524225	38.185920
2064.992072	344871.506532	38.190938
2066.871678	345503.129802	38.195956
2069.326123	346114.675569	38.200973
2071.466504	346742.000887	38.205991
2073.406589	347381.507769	38.211008
2075.247986	348012.190172	38.216026
2077.664406	348647.032853	38.221044
2080.373469	349266.337546	38.226061
2082.648997	349901.516054	38.231079
2084.887445	350534.636189	38.236096
2086.990409	351150.741414	38.241114
2089.080484	351784.934287	38.246132
2091.605499	352400.039101	38.251149
2093.734155	353051.768318	38.256167
2095.825592	353665.150623	38.261184
2098.174729	354293.352030	38.266202
2099.880593	354929.491427	38.271220
2101.722442	355559.179108	38.276237
2103.899559	356203.341918	38.281255
2106.333628	356838.520831	38.286272
2108.160227	357479.118883	38.291290
2110.237309	358120.249427	38.296308
2112.417045	358756.303917	38.301325
2114.602756	359398.563961	38.306343
2116.468784	360047.108283	38.311360
2118.510290	360668.186298	38.316378
2120.602188	361331.439376	38.321396
2122.711170	361981.282772	38.326413
2124.790209	362640.330127	38.331431
2126.704480	363306.827231	38.336448
2128.557605	363964.266144	38.341466
2130.681096	364614.748983	38.346484
2133.655426	365249.022080	38.351501
2136.232463	365908.338387	38.356519
2138.917905	366537.741844	38.361536
2141.648084	367175.828720	38.366554
2143.876037	367806.529734	38.371572
2146.365265	368413.205422	38.376589
2148.844937	369037.654828	38.381607
2151.306682	369637.263377	38.386624
2153.636301	370239.445988	38.391642
2156.021287	370818.425813	38.396660
2158.126752	371380.473518	38.401677
2160.248124	371949.891046	38.406695
2161.967535	372508.814497	38.411712
2164.469393	373074.423142	38.416730
2166.087367	373652.190887	38.421748
2167.856691	374222.011151	38.426765
2169.582435	374804.409307	38.431783
2171.358903	375392.039503	38.436800
2173.571931	375976.037310	38.441818
2175.108684	376590.798649	38.446836
2177.318127	377189.562420	38.451853
2179.031291	377807.392611	38.456871
2181.077928	378426.653018	38.461888
2183.623584	379040.164851	38.466906
2185.863811	379656.201239	38.471924
2188.371405	380286.002775	38.476941
2190.281133	380918.782013	38.481959
2192.338324	381553.502947	38.486976
2194.115527	382191.453030	38.491994
2195.867385	382835.607454	38.497012
2198.075470	383491.946476	38.502029
2199.853990	384157.116304	38.507047
2202.159754	384826.343939	38.512064
2204.634694	385495.073579	38.517082
2206.761576	386172.670027	38.522100
2208.892439	386837.752357	38.527117
2211.014021	387525.462604	38.532135
2213.576368	388203.274005	38.537152
2216.051945	388890.769654	38.542170
2217.580574	389584.414752	38.547188
2220.005606	390275.006755	38.552205
2222.269541	390966.345227	38.557223
2224.949428	391646.775472	38.562240
2227.554007	392340.663501	38.567258
2229.898361	393022.132708	38.572276
2232.389798	393705.590325	38.577293
2234.637603	394387.146384	38.582311
2237.117987	395069.890754	38.587328
2239.554519	395751.587700	38.592346
2241.929174	396428.311620	38.597364
2244.650418	397096.954016	38.602381
2247.272618	397764.558563	38.607399
2249.393249	398441.988127	38.612416
2251.508193	399118.642725	38.617434
2253.834493	399799.048231	38.622452
2256.338832	400461.212840	38.627469
2258.902922	401121.629239	38.632487
2260.920224	401787.188867	38.637504
2263.285598	402451.104567	38.642522
2265.138391	403131.028075	38.647540
2267.125211	403816.766571	38.652557
2269.111295	404498.662450	38.657575
2271.062097	405178.926009	38.662592
2273.232122	405866.231356	38.667610
2274.811414	406577.458981	38.672628
2277.223720	407272.214634	38.677645
2279.259209	407987.359251	38.682663
2282.134027	408683.624512	38.687680
2284.762155	409384.700863	38.692698
2287.173868	410087.492182	38.697716
2289.522427	410772.112089	38.702733
2292.167929	411475.664748	38.707751
2294.228293	412171.645348	38.712768
2296.909394	412854.992052	38.717786
2299.289566	413563.675630	38.722804
2301.338722	414246.128161	38.727821
2303.712487	414922.734525	38.732839
2306.363934	415587.424067	38.737856
2308.903280	416229.371039	38.742874
2311.256436	416871.915385	38.747892
2313.380559	417518.103219	38.752909
2315.687588	418174.856160	38.757927
2317.487241	418823.242740	38.762944
2319.476329	419486.345759	38.767962
2321.661811	420159.047464	38.772980
2323.984774	420829.834757	38.777997
2325.766425	421523.281008	38.783015
2327.476602	422211.351744	38.788032
2329.722691	422886.274931	38.793050
2331.753333	423605.348540	38.798068
2333.912066	424317.442665	38.803085
2336.163585	425049.806606	38.808103
2337.466922	425778.912476	38.813120
2340.080672	426515.223851	38.818138
2341.917138	427263.843675	38.823156
2344.245390	428017.068041	38.828173
2346.717102	428766.144263	38.833191
2348.995630	429536.037169	38.838208
2352.068560	430293.016462	38.843226
2354.460769	431071.498262	38.848244
2356.935684	431826.755450	38.853261
2359.307847	432595.521391	38.858279
2361.781147	433365.966595	38.863296
2364.269832	434128.841778	38.868314
2366.667464	434915.446169	38.873332
2368.900963	435693.598264	38.878349
2371.863639	436468.060989	38.883367
2373.956356	437242.590435	38.888384
2376.332792	438014.567013	38.893402
2379.111866	438807.655793	38.898420
2381.054845	439595.642245	38.903437
2383.419245	440379.027923	38.908455
2385.834121	441171.233441	38.913472
2388.282746	441967.554619	38.918490
2390.569154	442775.916644	38.923508
2392.738336	443571.366250	38.928525
2395.207537	444378.324071	38.933543
2397.568129	445195.591239	38.938560
2400.786488	445972.668493	38.943578
2403.514533	446772.918411	38.948596
2406.485897	447561.564634	38.953613
2409.016482	448346.207837	38.958631
2411.552800	449125.307780	38.963648
2414.264006	449915.933918	38.968666
2417.185708	450689.197487	38.973684
2419.309315	451465.902670	38.978701
2421.753936	452232.562761	38.983719
2424.253781	453015.420420	38.988736
2426.458688	453793.897624	38.993754
2428.855929	454581.315784	38.998772
2431.229161	455356.369185	39.003789
2433.936025	456130.832911	39.008807
2436.463377	456918.191366	39.013824
2438.834129	457688.404417	39.018842
2441.417231	458462.396163	39.023860
2444.162138	459223.742459	39.028877
2447.430915	459976.530666	39.033895
2450.170113	460734.180977	39.038912
2452.894110	461475.021328	39.043930
2455.494428	462225.762967	39.048948
2457.626025	462970.639301	39.053965
2460.121546	463713.557493	39.058983
2462.127414	464467.345567	39.064000
2464.423054	465215.952127	39.069018
2466.534610	465973.152847	39.074036
2468.654331	466685.948177	39.079053
2470.659782	467429.261909	39.084071
2472.630388	468177.808878	39.089088
2474.522363	468928.007604	39.094106
2476.380877	469691.119215	39.099124
2478.562126	470456.775014	39.104141
2480.848951	471220.968058	39.109159
2482.719088	472005.662684	39.114176
2485.143015	472809.534185	39.119194
2486.996921	473618.922056	39.124212
2489.391668	474425.255929	39.129229
2492.263971	475233.345724	39.134247
2494.938889	476078.411022	39.139264
2497.385920	476900.340348	39.144282
2500.092276	477729.060196	39.149300
2502.405401	478546.241185	39.154317
2505.104729	479384.232271	39.159335
2507.799361	480224.004120	39.164352
2510.375924	481055.171527	39.169370
2512.757618	481893.908223	39.174388
2515.073258	482750.240829	39.179405
2518.153073	483598.277213	39.184423
2520.612062	484450.465992	39.189440
2523.419869	485308.464243	39.194458
2525.907565	486155.316246	39.199476
2528.897161	487007.649198	39.204493
2531.904197	487851.608610	39.209511
2534.225306	488700.991803	39.214528
2536.586669	489544.118571	39.219546
2539.754119	490403.022394	39.224564
2542.645813	491240.882003	39.229581
2545.848600	492074.763750	39.234599
2548.742082	492927.582186	39.239616
2551.166114	493762.369036	39.244634
2553.427134	494594.064018	39.249652
2555.734161	495444.432280	39.254669
2558.578573	496277.059543	39.259687
2560.864898	497135.319481	39.264704
2563.153884	497967.450981	39.269722
2566.022053	498817.305836	39.274740
2568.712561	499673.402756	39.279757
2571.138147	500522.185001	39.284775
2573.455335	501405.697659	39.289792
2575.562783	502254.797379	39.294810
2577.936283	503119.445709	39.299828
2580.811575	503987.395757	39.304845
2583.589213	504850.676358	39.309863
2586.188591	505728.918767	39.314880
2589.117600	506598.184439	39.319898
2591.742560	507471.487868	39.324916
2594.580662	508340.019941	39.329933
2597.267489	509201.622859	39.334951
2599.210289	510081.805352	39.339968
2601.679504	510954.845314	39.344986
2604.092756	511825.376738	39.350004
2606.222513	512728.924939	39.355021
2608.822855	513627.606084	39.360039
2610.626160	514546.780689	39.365056
2613.130868	515460.242163	39.370074
2615.774096	516370.704699	39.375092
2617.723984	517286.570333	39.380109
2620.090556	518222.318691	39.385127
2622.112384	519177.366046	39.390144
2624.871487	520112.734118	39.395162
2627.710150	521065.363612	39.400180
2630.192495	522029.579810	39.405197
2632.996398	522986.831242	39.410215
2635.268855	523934.539487	39.415232
2637.986006	524864.637286	39.420250
2640.943546	525787.788542	39.425268
2643.447994	526720.375818	39.430285
2645.965649	527628.982175	39.435303
2648.853316	528566.830334	39.440320
2652.101708	529480.692529	39.445338
2655.133389	530386.679588	39.450356
2657.933987	531312.536514	39.455373
2660.747384	532220.712801	39.460391
2663.992521	533136.866760	39.465408
2666.362785	534049.584002	39.470426
2668.987891	534956.162041	39.475444
2671.600120	535882.818384	39.480461
2674.351411	536803.957149	39.485479
2677.099508	537719.501973	39.490496
2679.975538	538634.263013	39.495514
2682.880150	539551.627944	39.500532
2685.634830	540485.965399	39.505549
2688.385735	541412.997290	39.510567
2690.718217	542348.690789	39.515584
2693.052567	543282.108708	39.520602
2695.663490	544221.857981	39.525620
2698.109039	545185.916320	39.530637
2701.015420	546127.450959	39.535655
2703.538330	547096.696155	39.540672
2705.883720	548067.512324	39.545690
2708.720974	549028.725901	39.550708
2711.232890	550000.133338	39.555725
2713.753265	550985.196669	39.560743
2716.290748	551967.572200	39.565760
2719.311362	552958.494301	39.570778
2722.217805	553951.675402	39.575796
2724.932205	554948.987317	39.580813
2727.815549	555937.201417	39.585831
2730.382538	556947.206165	39.590848
2733.472223	557933.731923	39.595866
2737.018549	558917.396281	39.600884
2739.315896	559916.468254	39.605901
2742.277603	560908.874579	39.610919
2745.097034	561914.191109	39.615936
2747.819474	562920.150305	39.620954
2750.454851	563927.252402	39.625972
2752.814089	564942.911153	39.630989
2755.598066	565954.202318	39.636007
2758.237227	566956.148518	39.641024
2761.322196	567962.011139	39.646042
2764.782576	568966.729397	39.651060
2767.304776	569993.112371	39.656077
2770.592585	570974.456876	39.661095
2773.506398	571990.474514	39.666112
2776.125644	573001.942268	39.671130
2779.024425	573998.326820	39.676148
2781.883234	575020.384943	39.681165
2785.013754	576009.596893	39.686183
2787.690183	577016.920113	39.691200
2789.952787	578020.517711	39.696218
2793.161870	579034.364202	39.701236
2795.511394	580031.163250	39.706253
2798.449097	581032.751310	39.711271
2801.231248	582045.418892	39.716288
2803.910559	583061.380513	39.721306
2806.918380	584074.646357	39.726324
2809.091399	585087.665056	39.731341
2812.065824	586111.699192	39.736359
2815.256254	587117.863074	39.741376
2817.724033	588144.015332	39.746394
2821.197366	589135.576762	39.751412
2823.899898	590153.298336	39.756429
2826.645610	591131.933098	39.761447
2829.568112	592101.086986	39.766464
2832.815753	593046.656102	39.771482
2836.141329	593997.899614	39.776500
2838.507016	594957.842890	39.781517
2841.442518	595913.856812	39.786535
2844.201916	596887.556139	39.791552
2846.447296	597862.611955	39.796570
2848.807829	598838.118597	39.801588
2851.088466	599835.894053	39.806605
2853.895659	600830.041770	39.811623
2856.416304	601824.752432	39.816640
2858.514034	602841.378044	39.821658
2861.074457	603877.263311	39.826676
2863.575507	604932.038195	39.831693
2865.878863	605973.133179	39.836711
2868.701100	607036.571132	39.841728
2871.387216	608128.058665	39.846746
2874.091913	609200.722296	39.851764
2876.517647	610304.703679	39.856781
2879.373901	611419.413062	39.861799
2882.616170	612524.142785	39.866816
2885.039628	613656.961063	39.871834
2888.361333	614766.858360	39.876852
2891.167778	615902.336128	39.881869
2894.536865	617015.251522	39.886887
2897.992958	618139.940935	39.891904
2900.788667	619266.724089	39.896922
2903.802681	620412.202474	39.901940
2906.703461	621548.431897	39.906957
2909.574216	622679.999427	39.911975
2913.027824	623823.497192	39.916992
2916.149024	624960.882371	39.922010
2919.339450	626088.342876	39.927028
2922.595056	627239.905166	39.932045
2925.509578	628370.568578	39.937063
2929.080178	629490.514649	39.942080
2932.301090	630623.186247	39.947098
2935.337472	631739.487074	39.952116
2938.286808	632881.250524	39.957133
2940.893224	634011.962479	39.962151
2943.388554	635153.454232	39.967168
2946.059432	636294.343316	39.972186
2948.955482	637440.211479	39.977204
2951.876583	638592.337279	39.982221
2954.758725	639745.539037	39.987239
2957.737074	640897.249014	39.992256
2960.553767	642071.656435	39.997274
2963.802745	643218.172523	40.002292
2966.990912	644391.753884	40.007309
2969.795704	645539.429203	40.012327
2972.796580	646697.614150	40.017344
2975.781773	647870.428197	40.022362
2978.608909	649030.618266	40.027380
2981.362700	650206.339482	40.032397
2984.521197	651375.924742	40.037415
2987.701615	652546.964344	40.042432
2990.701143	653717.746604	40.047450
2993.939293	654891.091957	40.052468
2997.560603	656058.904282	40.057485
3000.437619	657229.440801	40.062503
3003.757960	658379.044544	40.067520
3006.450384	659560.191900	40.072538
3009.491958	660719.377787	40.077556
3011.983657	661883.146879	40.082573
3014.994150	663065.459892	40.087591
3017.791586	664234.870454	40.092608
3020.213905	665407.983813	40.097626
3022.724744	666568.249015	40.102644
3025.668438	667709.891030	40.107661
3029.036518	668850.480913	40.112679
3032.300190	669994.284614	40.117696
3035.051947	671142.810230	40.122714
3038.184405	672290.785666	40.127732
3041.097392	673446.564840	40.132749
3044.177942	674597.152289	40.137767
3047.459221	675755.271920	40.142784
3050.127772	676928.312489	40.147802
3053.096455	678107.717231	40.152820
3055.679361	679276.350486	40.157837
3058.773687	680463.734962	40.162855
3062.222894	681641.765957	40.167872
3064.791333	682855.660660	40.172890
3067.878474	684053.463459	40.177908
3071.213735	685261.697407	40.182925
3073.951062	686477.070648	40.187943
3077.332934	687682.443077	40.192960
3080.347598	688897.694866	40.197978
3083.368274	690120.178714	40.202996
3086.486364	691352.457038	40.208013
3089.546851	692579.613043	40.213031
3092.706168	693804.847829	40.218048
3095.430248	695062.135573	40.223066
3098.653762	696311.424744	40.228084
3101.788508	697563.528471	40.233101
3104.533148	698831.537381	40.238119
3108.372199	700079.845292	40.243136
3111.356562	701352.062737	40.248154
3114.968224	702616.308464	40.253172
3117.940651	703881.368463	40.258189
3120.950432	705149.360368	40.263207
3124.297068	706406.458272	40.268224
3127.338380	707689.581735	40.273242
3130.930249	708965.835304	40.278260
3134.564477	710215.890446	40.283277
3137.770955	711501.289742	40.288295
3141.145417	712768.049138	40.293312
3144.330043	714035.344231	40.298330
3147.999810	715280.838500	40.303348
3151.505655	716547.853041	40.308365
3154.951443	717804.196594	40.313383
3158.145283	719038.575027	40.318400
3161.403750	720301.007278	40.323418
3164.441745	721546.369401	40.328436
3167.569910	722798.453833	40.333453
3170.198252	724062.249271	40.338471
3173.442321	725314.824380	40.343488
3176.102895	726588.610054	40.348506
3179.213680	727858.714069	40.353524
3182.635695	729130.793716	40.358541
3185.083083	730405.355709	40.363559
3188.676279	731667.624181	40.368576
3192.132859	732955.452322	40.373594
3195.159822	734240.775967	40.378612
3198.298811	735510.619184	40.383629
3201.651554	736812.267053	40.388647
3204.663789	738094.114336	40.393664
3207.782350	739386.991086	40.398682
3210.639185	740677.924930	40.403700
3214.302791	741955.787384	40.408717
3217.467328	743265.145646	40.413735
3220.878960	744542.681131	40.418752
3223.416635	745856.299397	40.423770
3226.575639	747160.918078	40.428788
3229.563977	748473.086921	40.433805
3232.409170	749779.686408	40.438823
3235.300396	751065.706550	40.443840
3237.853818	752342.306166	40.448858
3240.728043	753625.046459	40.453876
3243.991791	754927.949976	40.458893
3246.669912	756232.157310	40.463911
3249.691973	757538.843418	40.468928
3252.514270	758871.775247	40.473946
3255.338735	760212.250402	40.478964
3259.017613	761547.279383	40.483981
3261.907518	762905.180860	40.488999
3265.069264	764255.758481	40.494016
3267.933201	765640.720134	40.499034
3270.770954	767030.200497	40.504052
3274.734201	768404.536283	40.509069
3279.296970	769771.146131	40.514087
3282.990286	771139.957790	40.519104
3286.927957	772511.670319	40.524122
3291.220992	773862.434473	40.529140
3294.415228	775233.664676	40.534157
3297.621968	776593.389817	40.539175
3301.153278	777940.287373	40.544192
3305.053093	779287.464629	40.549210
3308.432365	780638.453951	40.554228
3312.040090	781989.006658	40.559245
3314.665911	783347.957356	40.564263
3318.307526	784699.125817	40.569280
3321.641180	786070.691257	40.574298
3324.276974	787444.119618	40.579316
3327.435784	788823.032225	40.584333
3330.255037	790223.988756	40.589351
3333.390176	791615.598851	40.594368
3336.315057	793012.800951	40.599386
3339.004041	794438.816689	40.604404
3342.283707	795859.890752	40.609421
3345.746745	797294.603173	40.614439
3349.371282	798721.160689	40.619456
3352.668544	800173.227938	40.624474
3355.885481	801618.691469	40.629492
3359.581493	803068.129005	40.634509
3363.153674	804533.328086	40.639527
3366.544291	805971.344834	40.644544
3370.485749	807436.694970	40.649562
3373.988157	808887.430016	40.654580
3377.498148	810328.128155	40.659597
3381.619590	811766.514121	40.664615
3385.412856	813206.993685	40.669632
3389.167355	814633.201960	40.674650
3392.903247	816061.748180	40.679668
3396.565417	817480.188239	40.684685
3399.984879	818911.010754	40.689703
3403.193556	820321.111469	40.694720
3406.307731	821749.617173	40.699738
3409.233674	823176.870310	40.704756
3412.629728	824599.787052	40.709773
3415.089126	826037.374793	40.714791
3418.392516	827486.112013	40.719808
3421.383965	828957.391161	40.724826
3424.361597	830422.395838	40.729844
3427.967779	831889.354432	40.734861
3430.747331	833376.575010	40.739879
3433.755336	834869.454421	40.744896
3437.302397	836368.179821	40.749914
3440.121734	837873.879362	40.754932
3443.614500	839383.250464	40.759949
3446.875184	840908.309327	40.764967
3449.942119	842422.188091	40.769984
3453.512767	843949.676241	40.775002
3456.891808	845483.187713	40.780007
3460.555446	846930.889230	40.785012
3463.871062	848351.129881	40.790016
3467.200040	849704.609449	40.795021
3470.509186	850984.850309	40.800026
3473.380530	852216.017598	40.805031
3476.578706	853348.166461	40.810036
3478.826144	854447.850686	40.815040
3481.695694	855459.839503	40.820045
3484.392101	856408.634170	40.825050
3486.094387	857298.582505	40.830055
3489.014615	858116.893208	40.835060
3490.765389	858871.477738	40.840064
3493.111710	859566.250990	40.845069
3495.094120	860194.778153	40.850074
3496.905221	860774.551276	40.855079
3498.776874	861298.836914	40.860084
3500.559313	861773.313040	40.865088
3501.789332	862193.012172	40.870093
3503.417712	862563.232925	40.875098
3504.598003	862897.441132	40.880103
3505.773450	863181.572532	40.885108
3506.989059	863428.359786	40.890112
3507.877302	863643.505307	40.895117
3508.640738	863823.577361	40.900122
3509.580052	863962.989698	40.905127
3510.597822	864075.561943	40.910132
3511.401429	864170.965303	40.915136
3512.389377	864216.480471	40.920141
3513.267834	864242.867758	40.925146
3513.471428	864245.555622	40.930151
3514.521295	864220.114548	40.935156
3514.947005	864193.998679	40.940160
3515.702720	864114.958392	40.945165
3516.612318	864016.842640	40.950170
3517.138725	863912.568196	40.955175
3517.541763	863788.970898	40.960180
3518.073066	863649.215567	40.965184
3518.321135	863469.652564	40.970189
3518.848629	863297.814312	40.975194
3519.230969	863122.690193	40.980199
3519.266583	862904.749929	40.985204
3519.484464	862692.604476	40.990208
3519.940685	862467.871765	40.995213
3520.048582	862240.271607	41.000218
3520.029775	861992.850618	41.005223
3520.305609	861744.787705	41.010228
3520.821323	861495.508442	41.015232
3520.663470	861219.882343	41.020237
3520.975233	860952.626190	41.025242
3520.598357	860679.248249	41.030247
3520.792419	860403.332865	41.035252
3520.996862	860110.384306	41.040256
3521.011148	859821.635070	41.045261
3520.892477	859519.277583	41.050266
3520.804134	859229.058403	41.055271
3520.969969	858935.865511	41.060276
3520.753515	858644.277975	41.065280
3520.904163	858336.564971	41.070285
3520.954802	858016.886998	41.075290
3520.741915	857726.422720	41.080295
3520.634590	857400.025714	41.085300
3520.822817	857090.200961	41.090304
3520.764698	856775.730585	41.095309
3520.360811	856458.771064	41.100314
3520.364285	856146.593873	41.105319
3520.583270	855830.959213	41.110324
3520.054940	855526.331832	41.115328
3519.841906	855226.309282	41.120333
3520.229484	854907.485151	41.125338
3519.940146	854600.047399	41.130343
3519.934718	854274.928389	41.135348
3519.791830	853972.399885	41.140352
3519.721632	853658.941048	41.145357
3519.723576	853337.665801	41.150362
3519.292402	853040.201947	41.155367
3519.426059	852723.644026	41.160372
3519.200512	852415.503235	41.165376
3518.732980	852103.297155	41.170381
3519.064952	851794.644263	41.175386
3518.598903	851505.974557	41.180391
3518.800110	851193.125740	41.185396
3518.708030	850896.185236	41.190400
3518.466948	850593.313644	41.195405
3517.655602	850294.612341	41.200410
3517.797911	850006.065209	41.205415
3518.156273	849710.942347	41.210420
3518.018397	849418.127953	41.215424
3517.887886	849128.513646	41.220429
3517.686866	848833.149245	41.225434
3517.287433	848551.249413	41.230439
3517.343099	848249.092292	41.235444
3517.016971	847969.687620	41.240448
3517.054950	847688.456490	41.245453
3516.807581	847406.869959	41.250458
3516.666055	847135.583646	41.255463
3516.681154	846851.492612	41.260468
3516.696384	846586.784061	41.265472
3516.500476	846294.125790	41.270477
3516.196492	846023.598028	41.275482
3516.273692	845758.649510	41.280487
3516.212386	845480.357794	41.285492
3516.135557	845216.776613	41.290496
3516.080066	844932.610674	41.295501
3515.817079	844665.235037	41.300506
3515.474003	844408.586009	41.305511
3515.472515	844140.170108	41.310516
3515.596882	843886.640454	41.315520
3515.116071	843632.127720	41.320525
3515.373054	843372.802584	41.325530
3515.217663	843111.438133	41.330535
3514.976076	842857.001124	41.335540
3514.703464	842595.732240	41.340544
3514.424704	842331.381429	41.345549
3514.964217	842086.781643	41.350554
3514.588667	841845.736959	41.355559
3514.637683	841589.884546	41.360564
3514.162196	841353.422068	41.365568
3514.019678	841114.652346	41.370573
3514.209131	840875.087348	41.375578
3513.605557	840635.936627	41.380583
3513.818306	840392.398642	41.385588
3513.839732	840157.468402	41.390592
3513.606589	839923.205620	41.395597
3513.796683	839687.888825	41.400602
3513.389158	839455.491425	41.405607
3513.627991	839208.001004	41.410612
3513.223221	838994.272397	41.415616
3512.991544	838756.160917	41.420621
3513.013657	838542.054128	41.425626
3512.771836	838319.639634	41.430631
3512.628786	838092.126240	41.435636
3512.495211	837877.339704	41.440640
3512.654157	837675.185888	41.445645
3512.648417	837463.146035	41.450650
3512.285145	837251.158063	41.455655
3512.252625	837035.643436	41.460660
3511.947446	836831.245629	41.465664
3512.029283	836627.802542	41.470669
3512.355180	836416.112756	41.475674
3511.922131	836210.984126	41.480679
3511.929612	835990.986024	41.485684
3511.794742	835783.061093	41.490688
3511.638444	835579.868153	41.495693
3511.654519	835388.942482	41.500698
3511.409542	835195.466735	41.505703
3511.284799	834984.926948	41.510708
3511.030949	834793.149310	41.515712
3510.909998	834604.273498	41.520717
3511.220771	834410.926788	41.525722
3511.019771	834229.132818	41.530727
3510.960949	834035.200991	41.535732
3510.873443	833847.860034	41.540736
3510.720976	833671.169448	41.545741
3510.909835	833473.615330	41.550746
3510.920646	833291.320599	41.555751
3510.640511	833097.934277	41.560756
3510.751293	832920.789154	41.565760
3510.203004	832737.252324	41.570765
3510.372568	832551.638486	41.575770
3510.114016	832378.739537	41.580775
3510.375826	832188.118369	41.585780
3509.833046	832021.361937	41.590784
3509.935835	831843.602572	41.595789
3509.969524	831673.958121	41.600794
3510.150151	831508.778962	41.605799
3509.551896	831327.213167	41.610804
3509.520908	831158.982520	41.615808
3509.465839	830995.587722	41.620813
3509.549419	830830.944678	41.625818
3509.444298	830681.717329	41.630823
3509.077520	830504.438352	41.635828
3509.198085	830346.079180	41.640832
3509.386136	830184.333913	41.645837
3509.464060	830014.883177	41.650842
3508.991539	829860.127669	41.655847
3509.070007	829700.293952	41.660852
3508.930663	829553.000796	41.665856
3508.857662	829391.327710	41.670861
3508.994296	829239.291174	41.675866
3508.493538	829098.937117	41.680871
3508.516705	828922.723635	41.685876
3508.377821	828781.912223	41.690880
3508.177045	828643.844605	41.695885
3508.456321	828502.127523	41.700890
3508.149786	828370.620067	41.705895
3508.164976	828206.166361	41.710900
3507.857731	828081.935101	41.715904
3507.764689	827938.556588	41.720909
3507.914944	827795.574732	41.725914
3507.900433	827678.081183	41.730919
3507.798839	827525.799652	41.735924
3507.899952	827394.303177	41.740928
3507.485498	827258.929799	41.745933
3507.326476	827124.489146	41.750938
3507.433825	827000.511232	41.755943
3507.574783	826863.131844	41.760948
3507.572345	826733.545560	41.765952
3507.339982	826607.123145	41.770957
3507.338959	826477.678225	41.775962
3507.302172	826358.698157	41.780967
3507.552803	826233.948878	41.785972
3507.292717	826119.841021	41.790976
3507.250403	825990.637739	41.795981
3507.272801	825849.198936	41.800986
3507.102473	825731.891748	41.805991
3506.889031	825600.948943	41.810996
3506.932310	825484.971118	41.816000
3506.850903	825370.625251	41.821005
3506.896335	825248.775759	41.826010
3506.617325	825141.156897	41.831015
3506.839694	825018.442790	41.836020
3506.748575	824894.995689	41.841024
3506.585111	824781.973315	41.846029
3506.830100	824664.138606	41.851034
3506.592520	824550.195398	41.856039
3506.653333	824436.690069	41.861044
3506.363510	824327.837201	41.866048
3506.099176	824216.582164	41.871053
3506.472164	824118.521682	41.876058
3506.089299	824014.911503	41.881063
3506.325589	823902.101615	41.886068
3506.264097	823800.000048	41.891072
3506.138272	823688.028619	41.896077
3506.214279	823577.929389	41.901082
3505.911182	823473.857419	41.906087
3505.904887	823358.926304	41.911092
3506.054805	823256.585881	41.916096
3505.921398	823153.165628	41.921101
3506.488590	823051.242391	41.926106
3506.216518	822964.764898	41.931111
3505.678113	822845.265977	41.936116
3505.813607	822745.854722	41.941120
3505.702370	822647.998920	41.946125
3505.994553	822542.835978	41.951130
3505.538335	822444.985082	41.956135
3505.950158	822350.071423	41.961140
3505.729992	822249.879744	41.966144
3505.430810	822148.036394	41.971149
3505.833247	822055.272396	41.976154
3505.463418	821960.628661	41.981159
3505.520305	821870.364900	41.986164
3505.436667	821780.612250	41.991168
3505.583704	821678.394666	41.996173
3505.571623	821588.872236	42.001178
3505.261499	821494.799063	42.006183
3505.143351	821397.953286	42.011188
3505.299299	821308.008011	42.016192
3505.310007	821215.932801	42.021197
3505.313156	821126.499471	42.026202
3505.068778	821033.632036	42.031207
3505.061561	820953.053492	42.036212
3505.171166	820856.651559	42.041216
3505.028650	820782.698279	42.046221
3505.190988	820691.226868	42.051226
3504.702158	820608.864232	42.056231
3504.811971	820517.692652	42.061236
3504.896667	820447.612519	42.066240
3504.673156	820367.502865	42.071245
3505.024081	820283.285328	42.076250
3505.025485	820199.760401	42.081255
3504.885213	820116.208830	42.086260
3504.982755	820028.947111	42.091264
3505.052227	819949.958547	42.096269
3504.788963	819866.130495	42.101274
3504.423600	819796.704839	42.106279
3505.001002	819694.630526	42.111284
3504.522833	819620.915350	42.116288
3504.039648	819546.319337	42.121293
3504.642175	819469.145768	42.126298
3504.566583	819401.136352	42.131303
3504.774149	819303.129793	42.136308
3504.743085	819235.845421	42.141312
3504.446147	819170.414894	42.146317
3504.604429	819089.003497	42.151322
3504.207630	819011.744544	42.156327
3504.740986	818931.052479	42.161332
3504.755538	818860.233091	42.166336
3504.529489	818772.225160	42.171341
3504.595912	818710.254060	42.176346
3504.479839	818627.560788	42.181351
3504.399042	818549.167686	42.186356
3504.338016	818484.866211	42.191360
3504.050184	818407.924919	42.196365
3504.496172	818336.931027	42.201370
3504.198476	818276.239494	42.206375
3503.945287	818198.360121	42.211380
3504.286513	818128.507025	42.216384
3504.256104	818053.379206	42.221389
3504.651828	817992.962458	42.226394
3504.134017	817911.452277	42.231399
3503.965952	817838.694218	42.236404
3504.214242	817763.810931	42.241408
3504.018966	817697.370232	42.246413
3504.053104	817621.345836	42.251418
3503.856158	817572.770912	42.256423
3504.175735	817489.061733	42.261428
3504.087697	817437.628730	42.266432
3503.642306	817370.051143	42.271437
3504.152302	817307.455504	42.276442
3503.942040	817245.124775	42.281447
3503.769900	817164.184929	42.286452
3503.602657	817102.580087	42.291456
3503.648556	817035.162963	42.296461
3503.408856	816978.611208	42.301466
3503.429201	816924.463898	42.306471
3503.977307	816860.242288	42.311476
3503.900935	816805.816217	42.316480
3503.621072	816742.904804	42.321485
3503.700957	816676.849258	42.326490
3503.299857	816628.301104	42.331495
3503.579055	816569.555262	42.336500
3503.475382	816498.093879	42.341504
3503.349401	816457.822071	42.346509
3503.682774	816393.337610	42.351514
3503.476254	816335.453066	42.356519
3503.841392	816278.306180	42.361524
3503.530673	816214.513611	42.366528
3503.387494	816149.077132	42.371533
3503.414359	816089.291511	42.376538
3502.996099	816043.581697	42.381543
3502.956665	815991.591009	42.386548
3503.089636	815938.739161	42.391552
3503.214930	815886.426753	42.396557
3503.350227	815833.965400	42.401562
3502.719992	815790.345223	42.406567
3502.984567	815741.680999	42.411572
3502.822307	815687.211033	42.416576
3502.762917	815650.448827	42.421581
3502.999781	815589.938668	42.426586
3502.868293	815544.961657	42.431591
3502.938722	815504.651775	42.436596
3502.636778	815464.109191	42.441600
3502.567303	815418.484563	42.446605
3502.893287	815372.696555	42.451610
3502.562423	815327.359195	42.456615
3502.527950	815295.585552	42.461620
3502.614156	815252.578374	42.466624
3502.596450	815215.953826	42.471629
3502.613638	815165.612316	42.476634
3502.371098	815133.921149	42.481639
3502.531530	815085.465204	42.486644
3502.550920	815048.099104	42.491648
3502.420295	815006.056471	42.496653
3502.567360	814968.717870	42.501658
3502.300692	814932.475571	42.506663
3502.362294	814892.163471	42.511668
3502.469476	814853.263760	42.516672
3502.211424	814816.040009	42.521677
3502.401314	814774.824607	42.526682
3501.924610	814743.610906	42.531687
3502.662576	814711.119618	42.536692
3502.280047	814679.792166	42.541696
3502.138451	814639.365108	42.546701
3502.424672	814594.117045	42.551706
3502.336166	814568.519352	42.556711
3502.405181	814519.584669	42.561716
3502.617617	814485.317897	42.566720
3502.180937	814453.165768	42.571725
3502.388752	814421.984742	42.576730
3502.665287	814393.045038	42.581735
3502.434350	814356.499908	42.586740
3502.854123	814316.076391	42.591744
3502.668380	814275.654420	42.596749
3502.746825	814234.943817	42.601754
3502.785686	814176.559481	42.606759
3502.669687	814136.174160	42.611764
3502.620717	814097.001950	42.616768
3502.621851	814056.303002	42.621773
3502.676490	814014.468541	42.626778
3502.689899	813973.767073	42.631783
3502.627064	813928.523063	42.636788
3502.677521	813895.308489	42.641792
3502.213060	813850.766813	42.646797
3502.640747	813813.032744	42.651802
3502.648843	813780.706184	42.656807
3502.516614	813730.329578	42.661812
3502.504425	813696.438647	42.666816
3502.698041	813662.954456	42.671821
3502.632787	813612.565939	42.676826
3502.370895	813578.225751	42.681831
3502.449188	813526.980299	42.686836
3502.608325	813494.186669	42.691840
3502.292385	813469.307982	42.696845
3502.588317	813414.891092	42.701850
3502.049166	813403.910449	42.706855
3502.348784	813342.928946	42.711860
3502.313308	813306.149998	42.716864
3502.521348	813282.457834	42.721869
3502.555466	813242.679196	42.726874
3502.001047	813211.765076	42.731879
3502.177241	813160.304787	42.736884
3502.173670	813141.741165	42.741888
3501.991810	813101.311511	42.746893
3502.429336	813069.547591	42.751898
3502.295937	813037.583660	42.756903
3502.083913	813003.379280	42.761908
3502.313396	812971.992055	42.766912
3502.054457	812938.725769	42.771917
3502.294431	812902.536046	42.776922
3501.796092	812872.786759	42.781927
3502.050383	812843.942053	42.786932
3501.956784	812824.755586	42.791937
3501.866643	812786.954130	42.796941
3502.195620	812756.529222	42.801946
3501.873273	812736.792358	42.806951
3501.610624	812698.382008	42.811956
3501.951476	812687.157271	42.816961
3501.975812	812657.957761	42.821965
3502.123671	812619.087455	42.826970
3501.908472	812601.438963	42.831975
3501.709300	812562.772453	42.836980
3502.205294	812532.465990	42.841985
3502.138597	812509.061305	42.846989
3501.955816	812464.806986	42.851994
3502.026173	812453.969331	42.856999
3502.268690	812416.208984	42.862004
3502.227675	812391.085083	42.867009
3502.052923	812353.589069	42.872013
3502.073567	812309.104270	42.877018
3501.864835	812299.928965	42.882023
3502.083815	812261.289833	42.887028
3501.851708	812234.678166	42.892033
3501.617442	812200.571362	42.897037
3501.824990	812173.054214	42.902042
3501.584571	812146.639528	42.907047
3501.728791	812124.374528	42.912052
3502.033419	812099.192611	42.917057
3501.529505	812071.694258	42.922061
3501.841723	812047.735660	42.927066
3501.603028	812035.674485	42.932071
3501.756746	811997.387532	42.937076
3502.010105	811978.435460	42.942081
3501.656921	811945.718709	42.947085
3501.830456	811915.903527	42.952090
3501.683863	811895.449371	42.957095
3501.528696	811878.523977	42.962100
3501.782750	811851.340805	42.967105
3501.692385	811845.525833	42.972109
3501.841121	811803.368231	42.977114
3501.869882	811793.565211	42.982119
3502.129733	811746.832657	42.987124
3501.939299	811719.722172	42.992129
3501.517955	811703.820043	42.997133
3501.874127	811665.791828	43.002138
3501.812996	811647.331573	43.007143
3501.650064	811618.354398	43.012148
3501.658599	811599.392600	43.017153
3501.431681	811577.970838	43.022157
3501.640036	811553.145711	43.027162
3501.720947	811540.345089	43.032167
3501.635224	811504.985454	43.037172
3501.882746	811487.698787	43.042177
3501.653357	811458.927855	43.047181
3502.011223	811445.738473	43.052186
3501.998373	811414.481938	43.057191
3502.089952	811377.034634	43.062196
3501.985285	811348.193693	43.067201
3501.557020	811330.380994	43.072205
3502.092869	811297.759652	43.077210
3502.046698	811287.625270	43.082215
3501.960292	811260.152836	43.087220
3501.746650	811240.148711	43.092225
3501.637662	811215.570605	43.097229
3501.666686	811186.118994	43.102234
3501.330089	811165.791923	43.107239
3501.300217	811133.899937	43.112244
3501.500420	811125.341638	43.117249
3501.483545	811105.402699	43.122253
3501.833895	811079.131525	43.127258
3501.806394	811071.051642	43.132263
3501.421642	811027.115176	43.137268
3501.729841	811008.592347	43.142273
3501.286525	810976.718724	43.147277
3501.490812	810963.602703	43.152282
3501.580044	810954.180496	43.157287
3501.608979	810917.034963	43.162292
3501.507188	810902.107285	43.167297
3501.153150	810879.822272	43.172301
3501.746692	810872.668839	43.177306
3501.521632	810846.148549	43.182311
3501.405657	810821.717164	43.187316
3501.451988	810815.633793	43.192321
3501.204917	810779.071961	43.197325
3501.661390	810768.511013	43.202330
3501.442849	810749.731241	43.207335
3501.272966	810718.889365	43.212340
3501.818346	810709.342685	43.217345
3501.636825	810689.282642	43.222349
3501.750839	810673.632909	43.227354
3501.770975	810639.378337	43.232359
3502.079265	810629.527592	43.237364
3501.872380	810604.179382	43.242369
3501.761467	810578.276256	43.247373
3501.859212	810536.707198	43.252378
3501.513225	810519.515829	43.257383
3501.716875	810496.598679	43.262388
3501.496975	810480.856497	43.267393
3501.564642	810457.128580	43.272397
3501.534428	810436.846859	43.277402
3501.281986	810424.736071	43.282407
3501.345065	810401.106718	43.287412
3501.446311	810395.993977	43.292417
3501.171060	810363.305744	43.297421
3501.621038	810341.376556	43.302426
3501.120908	810332.295578	43.307431
3501.073979	810304.714766	43.312436
3501.033205	810281.837152	43.317441
3501.227772	810277.247987	43.322445
3501.251355	810266.806570	43.327450
3501.171383	810248.835646	43.332455
3501.516892	810241.967429	43.337460
3501.274629	810227.159411	43.342465
3501.248209	810202.760051	43.347469
3501.398562	810189.798434	43.352474
3500.962583	810183.352905	43.357479
3501.225569	810163.512114	43.362484
3501.139207	810139.563438	43.367489
3501.009640	810133.116395	43.372493
3501.327448	810134.289354	43.377498
3501.140533	810115.551621	43.382503
3501.321775	810093.959928	43.387508
3501.429901	810088.208761	43.392513
3501.355495	810058.867307	43.397517
3501.148851	810032.830853	43.402522
3501.223665	810035.465003	43.407527
3501.264304	810014.190248	43.412532
3501.571750	809983.756463	43.417537
3501.295561	809977.284416	43.422541
3501.546544	809955.729804	43.427546
3501.319028	809946.309368	43.432551
3501.136820	809938.057596	43.437556
3501.148401	809901.105390	43.442561
3501.191281	809901.882620	43.447565
3501.714568	809877.195523	43.452570
3501.347826	809869.268100	43.457575
3501.348884	809835.208642	43.462580
3501.453148	809826.174450	43.467585
3501.425013	809806.331564	43.472589
3501.526179	809806.560131	43.477594
3501.410020	809762.179177	43.482599
3501.328500	809754.057618	43.487604
3501.412227	809748.408198	43.492609
3501.311884	809742.053983	43.497613
3501.343056	809711.958533	43.502618
3500.895216	809725.117472	43.507623
3500.905860	809700.024100	43.512628
3501.202555	809674.785502	43.517633
3501.233737	809656.745696	43.522637
3501.127713	809646.275666	43.527642
3501.281978	809629.342696	43.532647
3501.048823	809604.975242	43.537652
3501.512175	809594.754407	43.542657
3501.126450	809586.878788	43.547661
3501.255348	809558.138795	43.552666
3501.270357	809563.625475	43.557671
3501.017143	809549.748944	43.562676
3501.241031	809521.287201	43.567681
3501.071943	809520.237053	43.572685
3501.361647	809510.485774	43.577690
3501.263760	809490.947512	43.582695
3501.207303	809465.080180	43.587700
3501.638242	809457.314941	43.592705
3501.227680	809445.963588	43.597709
3501.494455	809418.425529	43.602714
3501.077049	809414.181634	43.607719
3501.155748	809397.554592	43.612724
3501.599145	809366.997640	43.617729
3501.290272	809366.656632	43.622733
3501.355177	809339.935666	43.627738
3500.941217	809325.251981	43.632743
3501.126338	809323.555336	43.637748
3501.471800	809308.599497	43.642753
3501.052775	809275.488617	43.647757
3501.287922	809263.246431	43.652762
3501.210186	809261.789110	43.657767
3501.215471	809245.467854	43.662772
3501.581308	809228.352007	43.667777
3501.532980	809214.637087	43.672781
3501.450491	809185.146162	43.677786
3500.930983	809175.086592	43.682791
3501.146320	809171.326457	43.687796
3501.380406	809131.980882	43.692801
3501.190021	809129.267785	43.697805
3501.466307	809110.156914	43.702810
3501.279144	809094.406124	43.707815
3501.750238	809073.106538	43.712820
3501.294315	809060.340660	43.717825
3501.300591	809033.383089	43.722829
3501.242981	809008.935572	43.727834
3501.208739	809014.332783	43.732839
3501.246222	808996.535252	43.737844
3501.432669	808971.949378	43.742849
3501.140728	808976.947950	43.747853
3501.407793	808940.487589	43.752858
3501.457375	808947.096371	43.757863
3501.416713	808933.183569	43.762868
3501.290136	808889.582850	43.767873
3500.755649	808892.758925	43.772877
3501.396274	808873.636394	43.777882
3501.198296	808852.740408	43.782887
3501.281313	808835.768189	43.787892
3501.349229	808834.825937	43.792897
3501.317319	808812.873186	43.797901
3501.414944	808799.868599	43.802906
3501.364852	808795.024656	43.807911
3500.776547	808769.144255	43.812916
3501.416580	808750.266549	43.817921
3501.073701	808753.166055	43.822925
3501.205217	808734.813195	43.827930
3500.866075	808705.950643	43.832935
3501.111447	808697.136787	43.837940
3501.290004	808680.589578	43.842945
3501.174380	808687.274839	43.847949
3501.131451	808649.393538	43.852954
3501.107258	808640.869086	43.857959
3501.306869	808642.012767	43.862964
3501.520701	808615.411476	43.867969
3501.251888	808600.702315	43.872973
3501.405909	808591.315184	43.877978
3501.225981	808578.306876	43.882983
3501.183786	808549.100655	43.887988
3501.255912	808537.864338	43.892993
3501.097972	808533.626164	43.897997
3501.014585	808500.603276	43.903002
3500.776461	808505.299228	43.908007
3501.034669	808505.747055	43.913012
3501.353331	808501.381342	43.918017
3500.930184	808470.276884	43.923021
3501.049834	808462.071630	43.928026
3500.802890	808448.485915	43.933031
3500.907588	808446.949353	43.938036
3501.117488	808422.063536	43.943041
3500.992000	808418.898313	43.948045
3501.466997	808402.448653	43.953050
3501.180302	808396.565027	43.958055
3501.131474	808377.407624	43.963060
3501.542161	808357.586272	43.968065
3501.228899	808344.648497	43.973069
3501.154254	808322.848259	43.978074
3501.167225	808310.542928	43.983079
3501.080292	808300.508841	43.988084
3501.369643	808297.814425	43.993089
3500.799983	808278.595480	43.998093
3501.287639	808255.035802	44.003098
3500.935825	808256.466448	44.008103
3500.992243	808243.908751	44.013108
3501.094585	808210.706814	44.018113
3500.911225	808204.855018	44.023117
3500.812305	808208.743952	44.028122
3500.915513	808210.442787	44.033127
3500.904498	808213.925092	44.038132
3501.081633	808189.092842	44.043137
3500.710381	808183.762162	44.048141
3501.026398	808174.592868	44.053146
3501.027175	808176.847787	44.058151
3500.921969	808168.728236	44.063156
3501.030324	808140.769952	44.068161
3500.826716	808130.362682	44.073165
3501.131072	808122.224634	44.078170
3500.931423	808124.414546	44.083175
3500.670474	808128.134138	44.088180
3500.939294	808092.600319	44.093185
3500.639707	808081.130362	44.098189
3500.862921	808061.191974	44.103194
3500.864914	808073.348624	44.108199
3500.876475	808070.356741	44.113204
3501.168753	808068.446062	44.118209
3500.714599	808057.246622	44.123213
3500.698427	808040.484841	44.128218
3500.948795	808031.277150	44.133223
3500.859405	808034.429319	44.138228
3500.723490	808035.971507	44.143233
3500.618391	808028.341967	44.148237
3501.060310	808020.573297	44.153242
3501.116370	808010.515230	44.158247
3501.179065	807988.446203	44.163252
3501.464597	807992.517034	44.168257
3501.158535	807973.891066	44.173261
3501.246862	807937.454791	44.178266
3501.112374	807933.898662	44.183271
3500.773928	807931.062410	44.188276
3501.640183	807913.615748	44.193281
3500.964963	807900.344584	44.198285
3501.092401	807890.127521	44.203290
3501.293032	807883.525913	44.208295
3501.162737	807866.439359	44.213300
3501.080198	807847.138958	44.218305
3500.876979	807845.603959	44.223309
3500.998814	807838.328994	44.228314
3501.067176	807814.199592	44.233319
3500.993571	807797.348632	44.238324
3501.137803	807799.531026	44.243329
3500.827602	807804.141286	44.248333
3501.368748	807774.247411	44.253338
3501.346416	807758.662467	44.258343
3501.191220	807747.658380	44.263348
3501.227374	807734.808956	44.268353
3500.895608	807719.569021	44.273357
3501.133484	807712.323830	44.278362
3501.055785	807697.434171	44.283367
3501.169039	807690.111440	44.288372
3501.335800	807660.768956	44.293377
3501.022724	807656.359698	44.298381
3501.051970	807639.295319	44.303386
3501.008590	807632.439528	44.308391
3501.201381	807617.161984	44.313396
3500.923669	807609.413339	44.318401
3501.332712	807614.591572	44.323405
3501.299981	807588.664192	44.328410
3501.551319	807578.965507	44.333415
3501.168021	807562.851299	44.338420
3501.114834	807533.985706	44.343425
3501.185705	807510.296026	44.348429
3501.056854	807511.248887	44.353434
3501.104519	807517.173045	44.358439
3501.315806	807476.154897	44.363444
3501.599321	807463.705431	44.368449
3501.201203	807469.065751	44.373453
3501.402233	807453.051130	44.378458
3501.337046	807438.452989	44.383463
3500.985231	807432.383156	44.388468
3501.330335	807401.980686	44.393473
3500.794973	807391.479860	44.398477
3500.805587	807378.830070	44.403482
3500.920285	807370.624324	44.408487
3500.805381	807369.368814	44.413492
3501.181321	807349.011002	44.418497
3501.048238	807341.042131	44.423501
3501.342135	807335.699270	44.428506
3500.825309	807330.391894	44.433511
3500.986204	807308.304497	44.438516
3501.115387	807288.918620	44.443521
3500.960761	807287.816713	44.448525
3501.004654	807278.249822	44.453530
3501.178523	807266.847584	44.458535
3501.013051	807250.206507	44.463540
3501.158889	807232.337506	44.468545
3501.072344	807241.617726	44.473549
3500.862004	807216.943821	44.478554
3501.045024	807196.568307	44.483559
3501.113665	807201.704875	44.488564
3501.203550	807188.355319	44.493569
3500.737103	807193.825158	44.498573
3500.744928	807181.812795	44.503578
3501.041982	807156.025556	44.508583
3501.012375	807147.549157	44.513588
3501.094763	807145.231565	44.518593
3500.712894	807141.960899	44.523597
3500.976470	807136.230671	44.528602
3500.931732	807094.566043	44.533607
3500.778931	807097.876166	44.538612
3501.355554	807087.632946	44.543617
3500.932677	807089.075532	44.548621
3501.191670	807079.521959	44.553626
3501.321876	807051.408543	44.558631
3501.106344	807046.345475	44.563636
3501.235495	807035.489510	44.568641
3500.536349	807026.829084	44.573645
3500.588606	807001.326718	44.578650
3500.901425	807000.589011	44.583655
3501.035275	806995.664465	44.588660
3500.804917	806999.036437	44.593665
3501.009520	806983.804562	44.598669
3501.130105	806968.635520	44.603674
3501.007213	806957.624839	44.608679
3500.900963	806958.917243	44.613684
3501.116796	806953.096673	44.618689
3500.790789	806949.032274	44.623693
3501.039403	806921.928397	44.628698
3501.189341	806905.675775	44.633703
3501.211914	806897.092416	44.638708
3501.111043	806892.843818	44.643713
3500.874930	806874.595547	44.648717
3500.915215	806865.273813	44.653722
3501.094091	806862.597038	44.658727
3501.122905	806865.436106	44.663732
3501.202227	806843.948983	44.668737
3501.133975	806827.143778	44.673741
3500.955044	806820.456583	44.678746
3500.859753	806814.932284	44.683751
3500.753953	806800.535582	44.688756
3500.932047	806776.531532	44.693761
3500.964609	806761.621673	44.698765
3500.703096	806759.997969	44.703770
3500.955519	806761.378418	44.708775
3500.668756	806768.976255	44.713780
3500.858549	806749.431783	44.718785
3500.716501	806739.061277	44.723789
3500.797531	806720.858415	44.728794
3501.014584	806721.018975	44.733799
3500.897030	806720.842418	44.738804
3501.113845	806713.207412	44.743809
3500.829808	806720.265535	44.748813
3500.997500	806687.878933	44.753818
3501.024992	806688.806155	44.758823
3500.740907	806690.716251	44.763828
3501.320376	806677.137971	44.768833
3501.160369	806683.538321	44.773837
3500.802486	806648.492467	44.778842
3500.320616	806632.637443	44.783847
3500.607829	806633.178686	44.788852
3500.567755	806625.880074	44.793857
3500.502101	806633.196492	44.798861
3500.818398	806623.927025	44.803866
3500.588009	806635.830329	44.808871
3500.464989	806640.998888	44.813876
3500.737028	806635.168791	44.818881
3500.893149	806634.996183	44.823885
3500.630774	806607.926201	44.828890
3500.813856	806599.855358	44.833895
3500.761722	806584.076527	44.838900
3500.701862	806582.615685	44.843905
3500.474037	806584.761694	44.848909
3500.673919	806582.228440	44.853914
3500.842547	806576.807566	44.858919
3500.843826	806573.081273	44.863924
3500.903373	806574.052261	44.868929
3500.534816	806560.727964	44.873933
3500.542146	806548.812632	44.878938
3500.657722	806543.841742	44.883943
3500.881850	806534.587337	44.888948
3500.776936	806535.487358	44.893953
3500.652842	806538.694960	44.898957
3500.719958	806522.651194	44.903962
3500.709099	806530.792213	44.908967
3500.391413	806538.591518	44.913972
3501.045901	806530.099734	44.918977
3501.018760	806512.992805	44.923981
3500.837874	806486.105040	44.928986
3500.691928	806484.903510	44.933991
3500.547277	806498.705123	44.938996
3500.529713	806486.989906	44.944001
3500.457330	806502.544710	44.949005
3500.238436	806492.137457	44.954010
3500.513893	806489.934935	44.959015
3500.420638	806484.262941	44.964020
3501.083325	806489.449289	44.969025
3500.879491	806489.826273	44.974029
3500.672358	806467.796786	44.979034
3500.673624	806449.410219	44.984039
3500.523598	806456.348477	44.989044
3500.930764	806444.465167	44.994049
3500.862776	806441.289551	44.999053
3500.751503	806438.121063	45.004058
3500.797919	806435.171756	45.009063
3500.595486	806443.540557	45.014068
3500.874759	806430.011236	45.019073
3500.749424	806418.460747	45.024077
3500.622681	806396.319726	45.029082
3500.726226	806395.224179	45.034087
3500.609881	806401.372444	45.039092
3500.650698	806388.961006	45.044097
3500.641770	806410.487384	45.049101
3500.880679	806403.632894	45.054106
3500.491651	806409.580910	45.059111
3500.000356	806406.376940	45.064116
3500.470831	806403.946145	45.069121
3500.702646	806404.251376	45.074125
3500.668888	806408.915095	45.079130
3500.849749	806385.938875	45.084135
3500.593413	806378.430464	45.089140
3500.838471	806345.294030	45.094145
3500.720127	806365.563749	45.099149
3501.158579	806356.518959	45.104154
3500.629613	806357.537882	45.109159
3500.566320	806363.236159	45.114164
3500.550171	806356.227508	45.119169
3500.664997	806357.287484	45.124173
3500.788285	806350.746175	45.129178
3500.896927	806337.686062	45.134183
3500.731286	806320.650497	45.139188
3500.717753	806297.607938	45.144193
3500.771453	806315.593995	45.149197
3501.139083	806310.434324	45.154202
3501.259976	806308.502364	45.159207
3500.938240	806274.478310	45.164212
3500.980306	806262.458695	45.169217
3500.767139	806269.799798	45.174221
3500.792279	806257.979092	45.179226
3500.929069	806260.016110	45.184231
3500.856309	806250.368934	45.189236
3501.098050	806226.499572	45.194241
3500.827483	806224.239807	45.199245
3501.260510	806214.607336	45.204250
3501.102045	806218.997529	45.209255
3500.823295	806192.271828	45.214260
3501.140597	806172.018250	45.219265
3501.250276	806164.890612	45.224269
3501.194102	806159.800635	45.229274
3501.107762	806135.494667	45.234279
3500.705001	806136.149601	45.239284
3501.154226	806123.180081	45.244289
3500.924132	806130.720253	45.249293
3500.947623	806120.419609	45.254298
3500.866685	806089.885366	45.259303
3500.944826	806082.909937	45.264308
3500.978840	806078.197313	45.269313
3501.165470	806090.523207	45.274317
3500.733720	806060.389850	45.279322
3501.199880	806048.839377	45.284327
3500.952790	806036.131487	45.289332
3501.216475	806028.929307	45.294337
3501.272099	806023.771781	45.299341
3501.613028	805993.167620	45.304346
3501.318187	805986.253529	45.309351
3501.026699	805976.543926	45.314356
3501.018175	805960.266133	45.319361
3501.106527	805967.508860	45.324365
3501.156188	805961.273514	45.329370
3501.232852	805939.244615	45.334375
3500.991960	805921.386864	45.339380
3500.990276	805911.384261	45.344385
3501.012602	805910.351050	45.349389
3500.856562	805897.039488	45.354394
3500.826938	805877.822884	45.359399
3500.509034	805871.598964	45.364404
3500.988524	805867.254134	45.369409
3500.549058	805868.062242	45.374413
3500.660643	805852.499934	45.379418
3501.056263	805851.258122	45.384423
3500.955818	805851.912320	45.389428
3501.094314	805826.244272	45.394433
3500.808691	805818.740068	45.399437
3500.769253	805803.300596	45.404442
3501.048829	805813.454117	45.409447
3500.882376	805809.068541	45.414452
3500.904392	805798.718621	45.419457
3500.976390	805787.673955	45.424461
3500.524414	805771.223577	45.429466
3500.927653	805773.118783	45.434471
3500.415040	805777.420483	45.439476
3501.027196	805764.227308	45.444481
3500.843022	805773.966917	45.449485
3500.602812	805754.098153	45.454490
3500.801032	805737.442526	45.459495
3500.658949	805731.042410	45.464500
3501.089159	805725.675853	45.469505
3500.948766	805726.827002	45.474509
3500.769315	805723.865557	45.479514
3500.944770	805717.560234	45.484519
3501.049879	805706.264802	45.489524
3501.088989	805683.064398	45.494529
3500.777038	805677.280648	45.499533
3500.372094	805677.004289	45.504538
3500.891280	805675.153657	45.509543
3500.619047	805672.158435	45.514548
3500.683620	805674.648853	45.519553
3500.739870	805668.216009	45.524557
3500.844789	805638.286616	45.529562
3500.863858	805640.882614	45.534567
3500.703837	805633.602702	45.539572
3501.079136	805626.283644	45.544577
3501.015311	805642.574538	45.549581
3501.238979	805623.903942	45.554586
3501.320689	805605.648973	45.559591
3501.188644	805596.108715	45.564596
3501.033762	805578.432050	45.569601
3501.188119	805568.207096	45.574605
3501.474751	805544.180859	45.579610
3501.304286	805536.412190	45.584615
3501.357485	805516.984783	45.589620
3501.199997	805499.994872	45.594625
3500.780107	805499.524815	45.599629
3501.394276	805487.850949	45.604634
3501.302896	805456.825230	45.609639
3501.368561	805440.043604	45.614644
3501.371560	805430.775100	45.619649
3501.010289	805413.916617	45.624653
3501.383373	805404.734235	45.629658
3501.443462	805394.769742	45.634663
3501.306977	805372.381826	45.639668
3501.243823	805362.535664	45.644673
3501.472941	805357.790409	45.649677
3501.219389	805323.554247	45.654682
3501.085896	805317.838874	45.659687
3501.128165	805308.122386	45.664692
3501.307783	805281.808024	45.669697
3501.096476	805275.566002	45.674701
3501.231639	805262.450438	45.679706
3501.393452	805249.085262	45.684711
3500.924479	805237.834581	45.689716
3500.862124	805226.124588	45.694721
3501.139602	805226.079079	45.699725
3501.360598	805216.676301	45.704730
3500.982180	805187.952471	45.709735
3500.956211	805182.121195	45.714740
3501.207891	805166.681379	45.719745
3500.912802	805145.790050	45.724749
3500.878644	805136.380148	45.729754
3501.217711	805128.821331	45.734759
3500.903225	805119.702783	45.739764
3500.957420	805128.128992	45.744769
3501.009825	805107.621672	45.749773
3500.977647	805091.296674	45.754778
3501.389203	805105.058510	45.759783
3501.002479	805087.614930	45.764788
3501.078816	805054.990471	45.769793
3500.922608	805046.826571	45.774797
3500.766222	805043.174458	45.779802
3501.017105	805027.636380	45.784807
3501.006411	805009.100801	45.789812
3501.073861	804925.670354	45.794817
3500.811205	804797.566493	45.799821
3500.879405	804627.522393	45.804826
3501.064129	804393.156470	45.809831
3500.653810	804110.666987	45.814836
3500.246431	803755.865963	45.819841
3500.271032	803342.602647	45.824845
3499.686466	802880.113483	45.829850
3499.782919	802356.352615	45.834855
3499.415151	801789.844804	45.839860
3498.959891	801150.046007	45.844865
3498.691912	800457.796078	45.849869
3497.995646	799717.303439	45.854874
3497.657770	798897.058269	45.859879
3497.383626	798051.375370	45.864884
3497.260246	797126.028517	45.869889
3496.553437	796151.649887	45.874893
3495.839269	795111.770416	45.879898
3495.202510	794018.234124	45.884903
3494.661026	792870.718714	45.889908
3494.060375	791650.405018	45.894913
3493.025610	790380.611976	45.899917
3492.500566	789046.756285	45.904922
3491.781599	787668.780376	45.909927
3491.124698	786216.031984	45.914932
3490.582641	784699.228968	45.919937
3489.358595	783147.438263	45.924941
3488.114705	781513.538874	45.929946
3487.402886	779835.183761	45.934951
3486.567063	778113.140920	45.939956
3485.385606	776301.575155	45.944961
3484.482501	774447.010525	45.949965
3483.478951	772545.045068	45.954970
3482.067785	770592.048314	45.959975
3480.843187	768572.357520	45.964980
3480.306052	766491.903073	45.969985
3478.528082	764373.986951	45.974989
3477.528352	762183.665005	45.979994
3476.323707	759937.916683	45.984999
3475.099865	757653.794704	45.990004
3473.998400	755305.963518	45.995009
3472.867909	752907.581708	46.000013
3470.923089	750443.418981	46.005018
3469.681273	747942.822321	46.010023
3468.123129	745393.569363	46.015028
3466.769848	742771.742941	46.020033
3465.141647	740109.315758	46.025037
3463.532146	737390.268402	46.030042
3461.958564	734628.953338	46.035047
3460.436349	731826.420608	46.040052
3458.840108	728951.889049	46.045057
3457.064699	726043.369405	46.050061
3455.480443	723074.892499	46.055066
3453.715570	720067.789306	46.060071
3451.885532	717004.642439	46.065076
3449.946429	713899.154658	46.070081
3448.224616	710743.340245	46.075085
3446.281403	707547.804662	46.080090
3444.897101	704300.459873	46.085095
3442.589264	701001.949607	46.090100
3440.677332	697656.036923	46.095105
3439.037648	694268.121618	46.100109
3437.250423	690841.421334	46.105114
3435.427327	687343.028704	46.110119
3433.010009	683831.631885	46.115124
3431.230554	680252.073090	46.120129
3429.106025	676622.391059	46.125133
3426.699943	672966.014757	46.130138
3424.687278	669256.479751	46.135143
3422.366317	665501.788217	46.140148
3420.320054	661702.006067	46.145153
3418.074182	657880.495533	46.150157
3415.720255	654001.562337	46.155162
3413.695315	650070.881087	46.160167
3411.139068	646121.748129	46.165172
3409.123853	642121.922093	46.170177
3406.636638	638077.382967	46.175181
3403.899769	633989.261732	46.180186
3401.761020	629870.807203	46.185191
3398.986633	625700.966875	46.190196
3396.668415	621481.525775	46.195201
3394.411013	617243.294584	46.200205
3391.828511	612970.588450	46.205210
3389.629938	608653.890366	46.210215
3386.794703	604311.459543	46.215220
3384.259031	599906.883038	46.220225
3381.777240	595484.105028	46.225229
3379.016723	591012.079912	46.230234
3376.602928	586507.261899	46.235239
3373.677527	581974.407161	46.240244
3370.799942	577382.078211	46.245249
3367.918009	572776.893488	46.250253
3365.845332	568153.949105	46.255258
3363.331968	563477.351381	46.260263
3360.297871	558765.017515	46.265268
3357.598848	554007.675054	46.270273
3354.514934	549239.301026	46.275277
3351.819531	544420.500795	46.280282
3348.847663	539570.228765	46.285287
3345.845604	534710.949403	46.290292
3343.349869	529798.071709	46.295297
3340.307933	524869.670518	46.300301
3336.987034	519897.884950	46.305306
3334.143460	514892.635910	46.310311
3330.838875	509871.213914	46.315316
3327.925001	504823.940293	46.320321
3325.023052	499755.641294	46.325325
3321.884020	494646.186298	46.330330
3319.064437	489499.124818	46.335335
3315.787219	484351.085359	46.340340
3312.530200	479160.248538	46.345345
3309.213228	473954.130316	46.350349
3306.096497	468718.930596	46.355354
3302.925059	463448.775018	46.360359
3299.340671	458184.487790	46.365364
3296.263760	452880.375952	46.370369
3293.098647	447558.708481	46.375373
3289.816362	442225.146270	46.380378
3286.854070	436846.360747	46.385383
3283.449031	431469.532932	46.390388
3279.881910	426051.101207	46.395393
3276.632185	420630.425881	46.400397
3273.184842	415177.082466	46.405402
3270.089963	409711.928580	46.410407
3266.358755	404216.260692	46.415412
3262.749170	398712.133285	46.420417
3259.453238	393195.739593	46.425421
3255.985174	387667.194789	46.430426
3252.376875	382122.614276	46.435431
3249.003744	376557.419151	46.440436
3245.608495	370969.344994	46.445441
3241.802717	365376.571737	46.450445
3238.532156	359764.180242	46.455450
3234.995364	354124.171555	46.460455
3231.277027	348486.054414	46.465460
3227.705812	342840.964055	46.470465
3223.889213	337175.136911	46.475469
3220.012816	331500.822850	46.480474
3216.732257	325822.538002	46.485479
3212.748160	320135.499865	46.490484
3209.395211	314436.145278	46.495489
3205.478139	308718.857686	46.500493
3202.229039	303015.660614	46.505498
3198.581005	297279.415089	46.510503
3194.402251	291563.864076	46.515508
3190.769468	285814.992331	46.520513
3187.012803	280074.438498	46.525517
3183.081328	274320.865217	46.530522
3179.239484	268568.995068	46.535527
3175.100672	262818.378060	46.540532
3171.183697	257043.099464	46.545537
3167.552127	251288.223396	46.550541
3163.517752	245534.885029	46.555546
3159.684956	239767.700106	46.560551
3155.355570	234003.639270	46.565556
3151.535994	228238.330529	46.570561
3147.475203	222489.871253	46.575565
3143.513661	216730.622602	46.580570
3139.730801	210965.992321	46.585575
3135.693206	205151.635802	46.590580
3131.507043	199398.917460	46.595585
3127.456643	193670.582062	46.600589
3123.169613	187929.188741	46.605594
3118.979553	182197.675490	46.610599
3114.744433	176478.233682	46.615604
3111.018474	170765.674356	46.620609
3106.727022	165067.252244	46.625613
3102.197246	159371.926829	46.630618
3098.594641	153678.698390	46.635623
3093.762216	148018.685543	46.640628
3089.600814	142355.081655	46.645633
3085.262545	136697.161142	46.650637
3080.921232	131065.639198	46.655642
3076.621512	125446.473612	46.660647
3072.031608	119851.431051	46.665652
3067.797906	114259.440236	46.670657
3063.275523	108695.487468	46.675661
3058.731503	103155.104925	46.680666
3054.049927	97620.061569	46.685671
3049.183113	92126.260486	46.690676
3044.681620	86647.095993	46.695681
3039.689028	81195.944899	46.700685
3034.771296	75783.089229	46.705690
3029.675743	70398.839896	46.710695
3023.958585	65064.550391	46.715700
3017.941816	59784.134590	46.720705
3010.981018	54574.809436	46.725709
3000.838874	49508.690015	46.730714
2983.910097	44713.567750	46.735719
2967.028455	40111.299067	46.740724
2951.116783	35718.992671	46.745729
2935.394442	31597.774523	46.750733
2920.491393	27713.238458	46.755738
2905.810931	24118.991026	46.760743
2890.871044	20803.912551	46.765748
2877.019625	17775.139293	46.770753
2861.911586	15057.180329	46.775757
2844.143666	12701.606357	46.780762
2825.500912	10710.031341	46.785767
2806.784792	9063.307719	46.790772
2790.495551	7698.146682	46.795777
2777.802748	6602.263513	46.800781
2767.268947	5737.331890	46.805786
2759.745144	5071.542432	46.810791
2753.332095	4577.251179	46.815796
2748.776908	4221.172239	46.820801
2745.455263	3957.423401	46.825805
2742.485108	3783.319532	46.830810
2740.671686	3649.801841	46.835815
2738.873241	3554.307072	46.840820
2737.628499	3461.314144	46.845825
2736.449020	3389.445162	46.850829
2735.586589	3327.636956	46.855834
2734.841714	3247.008018	46.860839
2733.521131	3159.673069	46.865844
2732.016027	3044.621112	46.870849
2730.332636	2923.364173	46.875853
2728.652888	2786.728643	46.880858
2726.953363	2631.228831	46.885863
2724.738785	2478.457997	46.890868
2722.618363	2297.139140	46.895873
2720.164753	2118.236392	46.900877
2717.519276	1925.809148	46.905882
2714.936443	1707.224517	46.910887
2711.796671	1504.695974	46.915892
2708.773574	1291.136651	46.920897
2705.637012	1081.239554	46.925901
2702.278326	873.827036	46.930906
2699.045276	648.452769	46.935911
2695.582709	438.889104	46.940916
2691.787527	233.365457	46.945921
2684.134069	140.610114	46.950925
2671.959248	203.311971	46.955930
2665.492850	206.604583	46.960935
2661.898088	213.216622	46.965940
2660.159144	220.236095	46.970945
2658.822027	213.548373	46.975949
2656.443151	210.019054	46.980954
2654.193318	200.279421	46.985959
2650.666303	209.769353	46.990964
2647.609862	200.230394	46.995969
2644.647466	211.451854	47.000973
2640.655842	205.170144	47.005978
2637.499150	195.291363	47.010983
2633.998816	195.518353	47.015988
2630.403769	201.447226	47.020993
2627.253415	204.574439	47.025997
2623.909994	211.557153	47.031002
2620.866327	205.346861	47.036007
2617.545426	209.959899	47.041012
2613.632438	200.622172	47.046017
2610.865973	197.796095	47.051021
2607.672073	207.159391	47.056026
2604.588567	197.099850	47.061031
2600.720790	206.624082	47.066036
2597.337761	201.792196	47.071041
2593.960701	194.322742	47.076045
2590.017213	196.159054	47.081050
2586.699610	197.407452	47.086055
2583.433220	200.082317	47.091060
2579.802015	200.896034	47.096065
2577.223687	200.664782	47.101069
2573.442670	204.412882	47.106074
2570.536488	193.832006	47.111079
2566.787687	196.488353	47.116084
2563.372303	191.257021	47.121089
2559.553565	195.837424	47.126093
2556.089746	204.050569	47.131098
2553.145829	180.469209	47.136103
2548.978846	192.884981	47.141108
2545.504625	188.744376	47.146113
2542.649865	194.147203	47.151117
2538.863861	192.423183	47.156122
2535.253646	196.652812	47.161127
2531.256718	202.821733	47.166132
2528.085486	195.748431	47.171137
2525.449149	193.116503	47.176141
2521.424289	186.244051	47.181146
2518.697838	177.939649	47.186151
2515.439252	188.709960	47.191156
2511.577833	191.865671	47.196161
2507.939551	190.457684	47.201165
2504.347328	190.986294	47.206170
2500.863825	183.148095	47.211175
2497.649416	184.094979	47.216180
2494.350576	186.011996	47.221185
2490.838452	179.422426	47.226189
2486.927073	177.482523	47.231194
2483.570301	183.636566	47.236199
2480.080695	187.411732	47.241204
2476.526683	184.660130	47.246209
2473.273945	177.323465	47.251213
2469.770611	179.049960	47.256218
2467.055858	175.441827	47.261223
2462.999912	188.651880	47.266228
2459.504412	191.098193	47.271233
2456.083637	181.752020	47.276237
2452.071820	181.812447	47.281242
2448.892903	177.944532	47.286247
2445.096939	182.578154	47.291252
2441.609143	177.579530	47.296257
2439.102237	182.273476	47.301261
2435.138174	185.438157	47.306266
2431.466026	166.656809	47.311271
2427.852372	179.072040	47.316276
2424.135972	169.156837	47.321281
2421.150162	176.257928	47.326285
2417.847260	182.290147	47.331290
2414.235058	178.588313	47.336295
2410.774844	179.182018	47.341300
2407.015407	178.293378	47.346305
2403.978444	178.028504	47.351309
2400.378253	180.273180	47.356314
2396.744790	167.283207	47.361319
2393.322467	176.221903	47.366324
2389.765715	168.966399	47.371329
2386.042611	170.278990	47.376333
2382.279158	182.782874	47.381338
2379.361318	183.621013	47.386343
2376.350689	166.699854	47.391348
2372.811236	166.353297	47.396353
2369.117444	162.340653	47.401357
2365.096060	181.429287	47.406362
2362.078011	170.927062	47.411367
2358.451641	166.034509	47.416372
2354.681576	171.450904	47.421377
2351.329427	172.462592	47.426381
2347.708772	176.773439	47.431386
2344.461972	163.284646	47.436391
2340.808571	169.467925	47.441396
2337.165183	168.633980	47.446401
2333.867572	164.257079	47.451405
2330.820744	175.411818	47.456410
2327.591182	176.714866	47.461415
2323.356792	168.432033	47.466420
2319.714675	162.916794	47.471425
2316.457349	161.835685	47.476429
2312.928993	177.243334	47.481434
2309.497740	168.456898	47.486439
2305.916735	168.287807	47.491444
2302.638816	170.725432	47.496449
2299.186338	168.723464	47.501453
2295.910756	169.698278	47.506458
2292.404271	161.288218	47.511463
2288.403590	163.035352	47.516468
2284.850838	156.844576	47.521473
2281.794406	165.379825	47.526477
2277.992911	168.319562	47.531482
2274.834440	168.814232	47.536487
2271.006402	161.228338	47.541492
2267.287809	164.606365	47.546497
2264.140634	159.860564	47.551501
2260.537504	161.689937	47.556506
2257.060819	164.460188	47.561511
2254.059233	169.785301	47.566516
2250.033073	168.318093	47.571521
2246.648097	162.133998	47.576525
2243.166416	159.354408	47.581530
2240.052949	158.459355	47.586535
2236.196209	164.787698	47.591540
2232.203245	160.195913	47.596545
2229.281494	158.655386	47.601549
2225.740420	173.842778	47.606554
2222.306733	163.539217	47.611559
2218.874453	154.979333	47.616564
2215.066891	152.786662	47.621569
2211.706101	152.879542	47.626573
2208.154199	157.310420	47.631578
2204.893072	151.387103	47.636583
2201.165552	149.054559	47.641588
2197.650220	169.335628	47.646593
2194.274266	158.468986	47.651597
2190.238365	154.305288	47.656602
2186.997680	149.396377	47.661607
2183.904283	159.128862	47.666612
2180.303473	172.636087	47.671617
2176.799893	156.384077	47.676621
2173.272518	157.160634	47.681626
2170.112820	150.755722	47.686631
2166.336020	155.112129	47.691636
2162.883652	158.838363	47.696641
2159.091350	147.733987	47.701645
2155.746896	169.770836	47.706650
2152.380887	149.260815	47.711655
2148.574405	150.701421	47.716660
2145.103888	153.072908	47.721665
2142.071833	141.635176	47.726669
2138.339230	149.412805	47.731674
2134.630682	158.190033	47.736679
2131.152928	159.839648	47.741684
2127.767851	159.123916	47.746689
2124.481055	145.502261	47.751693
2120.606406	151.933843	47.756698
2117.240956	153.004161	47.761703
2113.862639	156.171136	47.766708
2109.888963	147.323346	47.771713
2106.904895	140.155083	47.776717
2103.456788	154.515591	47.781722
2100.104460	148.856189	47.786727
2096.512638	154.692784	47.791732
2092.498478	148.247027	47.796737
2089.208837	145.394501	47.801741
2085.527674	160.137980	47.806746
2082.441168	148.958271	47.811751
2078.945559	155.540355	47.816756
2075.267543	146.809367	47.821761
2071.859034	158.207236	47.826765
2067.911468	154.081032	47.831770
2064.883171	156.244644	47.836775
2061.674089	148.736144	47.841780
2057.854720	152.333732	47.846785
2054.349380	147.026945	47.851789
2050.375676	158.146603	47.856794
2047.509343	147.171422	47.861799
2044.044188	156.333856	47.866804
2040.400476	147.101074	47.871809
2036.851288	147.539241	47.876813
2033.230760	146.862592	47.881818
2029.802227	159.403784	47.886823
2026.269007	148.860842	47.891828
2022.769586	151.235770	47.896833
2019.330961	156.723623	47.901837
2015.876648	157.003982	47.906842
2012.293852	144.788870	47.911847
2008.847888	149.900467	47.916852
2005.118850	153.467098	47.921857
2001.805691	146.375467	47.926861
1997.897532	144.592467	47.931866
1994.640493	136.959914	47.936871
1991.752822	148.124684	47.941876
1988.239639	150.351542	47.946881
1984.385291	142.923288	47.951885
1980.700632	148.088578	47.956890
1977.226437	146.191084	47.961895
1973.894253	146.260608	47.966900
1970.277196	146.326812	47.971905
1966.957051	146.904124	47.976909
1963.050265	147.764285	47.981914
1959.871327	145.780403	47.986919
1956.194272	147.132369	47.991924
1952.698943	145.588316	47.996929
1949.579871	138.853316	48.001933
1946.142398	145.766922	48.006938
1942.152059	142.531341	48.011943
1939.004209	145.929904	48.016948
1935.361820	141.901325	48.021953
1931.827082	140.290383	48.026957
1928.207475	147.620096	48.031962
1924.912464	152.133025	48.036967
1921.319974	144.840577	48.041972
1917.842353	139.499596	48.046977
1914.498842	137.522465	48.051981
1910.471438	143.238807	48.056986
1907.048952	138.803404	48.061991
1903.682547	146.203529	48.066996
1900.195848	138.191290	48.072001
1897.100516	138.668107	48.077005
1893.202302	136.321072	48.082010
1889.837941	137.079944	48.087015
1886.124339	146.302954	48.092020
1882.877591	144.611769	48.097025
1879.804068	139.507320	48.102029
1875.972382	140.371021	48.107034
1872.178743	133.104195	48.112039
1868.617341	142.743893	48.117044
1864.941214	146.041203	48.122049
1861.896800	137.611600	48.127053
1858.473709	145.757484	48.132058
1854.675969	137.356865	48.137063
1851.381747	135.873608	48.142068
1847.501617	140.490007	48.147073
1844.182661	131.203970	48.152077
1841.065606	145.316268	48.157082
1837.226361	135.445291	48.162087
1834.018749	139.072974	48.167092
1830.420194	138.892804	48.172097
1827.170852	135.867222	48.177101
1823.372411	140.000342	48.182106
1819.705576	137.053510	48.187111
1816.215955	135.386347	48.192116
1812.881610	136.296577	48.197121
1809.271701	129.688411	48.202125
1805.177833	146.845576	48.207130
1802.204928	135.218615	48.212135
1798.566409	128.366950	48.217140
1795.132484	134.905223	48.222145
1792.087151	136.897716	48.227149
1788.237903	138.234172	48.232154
1784.877714	137.369075	48.237159
1781.093176	135.117298	48.242164
1777.569643	135.339242	48.247169
1774.782184	135.398698	48.252173
1770.780095	139.723100	48.257178
1767.004177	132.354163	48.262183
1763.738794	134.520505	48.267188
1760.164771	135.066988	48.272193
1757.319035	123.411975	48.277197
1753.235230	132.493962	48.282202
1749.937271	129.834571	48.287207
1745.919400	132.630605	48.292212
1742.180989	131.431129	48.297217
1738.984796	125.862875	48.302221
1735.597865	133.619250	48.307226
1732.408178	127.234315	48.312231
1728.975017	133.544784	48.317236
1725.359344	143.563562	48.322241
1721.853182	133.652500	48.327245
1717.999093	139.991782	48.332250
1715.129406	132.275044	48.337255
1711.309778	134.398091	48.342260
1707.139947	137.336032	48.347265
1704.057065	132.676981	48.352269
1700.649350	133.676716	48.357274
1697.540853	132.588500	48.362279
1693.589527	131.590520	48.367284
1690.330797	134.022371	48.372289
1686.814444	119.114192	48.377293
1683.006754	133.421678	48.382298
1679.498843	135.543820	48.387303
1675.965528	132.036063	48.392308
1672.636362	134.893713	48.397313
1669.511071	122.040001	48.402317
1666.068618	130.505051	48.407322
1662.569473	125.403067	48.412327
1658.871736	136.154332	48.417332
1654.802517	124.206978	48.422337
1651.699592	125.538646	48.427341
1647.951201	125.623625	48.432346
1644.701085	116.814808	48.437351
1641.495727	123.884583	48.442356
1637.451046	136.564855	48.447361
1634.324658	121.791155	48.452365
1630.454795	127.396493	48.457370
1627.026137	119.952685	48.462375
1623.762952	124.029835	48.467380
1619.915942	127.405377	48.472385
1616.597851	119.761996	48.477389
1612.959234	138.114132	48.482394
1609.413097	125.813818	48.487399
1606.099211	114.911755	48.492404
1602.605111	120.681715	48.497409
1599.263557	129.183712	48.502413
1595.535709	131.884216	48.507418
1592.190288	128.245065	48.512423
1588.813384	117.247648	48.517428
1585.063154	123.351221	48.522433
1581.375385	127.847804	48.527437
1578.051623	130.922735	48.532442
1574.646147	131.737077	48.537447
1571.203719	131.072118	48.542452
1567.450138	127.913122	48.547457
1564.536697	122.502916	48.552461
1560.294610	125.744592	48.557466
1557.332047	124.658502	48.562471
1553.923185	132.646763	48.567476
1550.028348	129.848005	48.572481
1546.959370	124.583244	48.577485
1542.707720	126.682862	48.582490
1539.538181	127.551517	48.587495
1536.099463	119.549042	48.592500
1532.475729	118.698553	48.597505
1528.941567	123.105287	48.602509
1525.655421	124.422651	48.607514
1522.265934	123.766640	48.612519
1518.368891	122.212742	48.617524
1514.760202	114.241390	48.622529
1511.584096	115.185134	48.627533
1508.336097	119.871013	48.632538
1504.644100	118.514342	48.637543
1500.976352	117.391832	48.642548
1497.446828	126.576525	48.647553
1494.040862	118.138618	48.652557
1490.346888	122.397908	48.657562
1487.071702	122.586803	48.662567
1483.964146	120.355968	48.667572
1479.828600	114.573006	48.672577
1476.431291	107.207976	48.677581
1472.860349	121.620106	48.682586
1469.142464	115.698570	48.687591
1466.011440	116.104409	48.692596
1462.546892	124.519315	48.697601
1459.561241	110.896932	48.702605
1455.515983	122.363576	48.707610
1452.000528	117.138908	48.712615
1448.848697	114.446969	48.717620
1444.983194	128.111261	48.722625
1441.595283	112.417747	48.727629
1437.782059	118.628764	48.732634
1434.199650	117.391772	48.737639
1430.848371	129.450190	48.742644
1427.360965	117.859722	48.747649
1424.010169	117.472827	48.752653
1420.254874	116.118460	48.757658
1417.393213	110.618290	48.762663
1413.716249	104.132817	48.767668
1409.913731	116.580525	48.772673
1406.969524	114.701516	48.777677
1402.933195	120.795072	48.782682
1399.410239	119.820088	48.787687
1396.214333	115.501472	48.792692
1392.485460	118.514300	48.797697
1388.894155	118.703818	48.802701
1385.014828	119.405455	48.807706
1381.681572	115.365238	48.812711
1378.608236	109.103556	48.817716
1374.810515	120.321606	48.822721
1371.580241	114.059980	48.827725
1367.877071	120.004939	48.832730
1364.597524	108.895994	48.837735
1361.244423	111.136379	48.842740
1357.609708	123.291226	48.847745
1354.147428	120.034845	48.852749
1350.024231	115.944284	48.857754
1346.701424	122.472881	48.862759
1343.419978	111.538885	48.867764
1339.778446	111.576695	48.872769
1336.615264	107.543652	48.877773
1333.035852	124.307069	48.882778
1329.529831	106.200319	48.887783
1325.906904	114.420226	48.892788
1322.087889	125.755667	48.897793
1319.001348	115.900007	48.902797
1315.077847	122.650300	48.907802
1311.724527	113.131596	48.912807
1308.523579	109.354701	48.917812
1304.835777	118.602294	48.922817
1301.593316	105.000494	48.927821
1297.816018	122.328842	48.932826
1294.204081	121.386358	48.937831
1291.159453	110.336450	48.942836
1287.361932	116.119632	48.947841
1284.057599	108.489364	48.952845
1280.507088	116.582007	48.957850
1276.631060	121.977406	48.962855
1273.277506	112.951758	48.967860
1270.061992	123.535968	48.972865
1266.576605	123.156961	48.977869
1262.603992	124.898332	48.982874
1259.219158	114.161007	48.987879
1255.841867	108.810352	48.992884
1252.448517	122.664638	48.997889
1249.113490	111.335637	49.002893
1245.694785	126.995312	49.007898
1241.648895	119.446230	49.012903
1238.368993	112.818362	49.017908
1234.787124	108.574590	49.022913
1231.416376	106.633176	49.027917
1227.636352	118.941101	49.032922
1224.150051	118.962423	49.037927
1220.542385	118.805874	49.042932
1217.251059	114.813675	49.047937
1213.833965	102.126213	49.052941
1210.653873	106.553273	49.057946
1206.987362	105.824363	49.062951
1203.587523	109.073222	49.067956
1199.460941	118.471034	49.072961
1196.328020	122.438759	49.077965
1192.502514	115.855894	49.082970
1189.357334	108.215882	49.087975
1186.157114	106.933000	49.092980
1182.152974	116.681166	49.097985
1178.861802	112.495988	49.102989
1174.970984	119.973488	49.107994
1171.618452	125.417093	49.112999
1168.387094	117.496426	49.118004
1164.657414	113.801261	49.123009
1161.425622	111.390912	49.128013
1157.818183	116.126307	49.133018
1154.285783	100.128612	49.138023
1150.474118	105.926426	49.143028
1147.102556	116.010491	49.148033
1143.800004	119.135486	49.153037
1140.056477	119.861704	49.158042
1136.751891	112.454328	49.163047
1133.398409	101.484408	49.168052
1129.740623	121.289719	49.173057
1126.386756	110.623234	49.178061
1122.437217	115.345863	49.183066
1119.251706	121.884544	49.188071
1116.030203	112.374384	49.193076
1111.904525	116.917141	49.198081
1108.823488	110.312158	49.203085
1105.191734	117.705388	49.208090
1101.836428	119.083496	49.213095
1098.496286	104.969832	49.218100
1094.554459	111.480557	49.223105
1091.328062	108.467244	49.228109
1087.237332	114.087802	49.233114
1084.108283	97.705496	49.238119
1081.001607	104.993893	49.243124
1077.169399	105.299507	49.248129
1073.916345	103.658790	49.253133
1069.991981	106.061399	49.258138
1066.464217	113.175442	49.263143
1063.155332	101.374607	49.268148
1059.471077	109.944432	49.273153
1056.214882	104.085737	49.278157
1052.847537	104.892358	49.283162
1049.228486	111.806011	49.288167
1045.878358	104.708989	49.293172
1041.878433	109.044164	49.298177
1038.829016	109.693232	49.303181
1035.164244	112.954240	49.308186
1031.463485	102.629815	49.313191
1028.250247	106.477087	49.318196
1024.429457	104.711600	49.323201
1021.211791	98.608604	49.328205
1017.619392	112.679428	49.333210
1014.138966	110.016695	49.338215
1010.410816	101.096957	49.343220
1006.981305	112.677510	49.348225
1004.006084	101.822801	49.353229
1000.038385	112.386360	49.358234
996.507157	95.097947	49.363239
993.379313	104.226283	49.368244
989.467439	116.593861	49.373249
986.501304	104.943169	49.378253
982.260471	96.147858	49.383258
978.951900	91.420779	49.388263
975.720873	96.718906	49.393268
971.926630	113.436512	49.398273
968.466597	93.609250	49.403277
965.148810	101.635875	49.408282
961.498806	100.901316	49.413287
958.251546	95.660378	49.418292
954.718062	97.675507	49.423297
951.762021	97.140795	49.428301
947.894744	95.813078	49.433306
943.952237	93.878018	49.438311
940.805403	97.900134	49.443316
936.816494	108.271387	49.448321
933.283604	107.635698	49.453325
930.051223	105.354311	49.458330
926.484260	93.339177	49.463335
923.343872	92.404770	49.468340
919.095124	106.588734	49.473345
915.813424	99.859434	49.478349
912.602908	103.922169	49.483354
909.223915	85.013697	49.488359
905.634908	95.816062	49.493364
901.988463	99.917039	49.498369
899.055859	104.524948	49.503373
894.938972	104.442492	49.508378
891.267633	101.686451	49.513383
888.213224	92.864211	49.518388
884.186793	101.115120	49.523393
881.198068	97.536828	49.528397
877.475458	107.303862	49.533402
873.607235	98.997906	49.538407
870.342646	96.190895	49.543412
866.908145	96.072240	49.548417
863.844857	97.503365	49.553421
860.209340	92.623945	49.558426
856.467475	100.650000	49.563431
852.842118	95.526110	49.568436
849.347904	98.524933	49.573441
846.184077	93.676057	49.578445
842.387591	99.766404	49.583450
838.915741	105.600210	49.588455
835.619986	96.640858	49.593460
831.681743	91.129721	49.598465
828.415981	89.849550	49.603469
825.031501	100.658332	49.608474
821.510449	95.782625	49.613479
817.925301	96.739670	49.618484
814.626870	100.455484	49.623489
811.387230	90.384288	49.628493
807.404345	102.201513	49.633498
803.753273	96.709072	49.638503
800.817838	96.888757	49.643508
796.652447	96.868732	49.648513
793.551053	97.472527	49.653517
789.671517	109.782166	49.658522
786.154514	92.163225	49.663527
782.950232	96.654046	49.668532
779.184017	87.664885	49.673537
776.130630	93.267420	49.678541
772.573958	87.763556	49.683546
768.794253	92.342993	49.688551
765.393786	93.868911	49.693556
761.810745	93.549111	49.698561
758.510010	90.671373	49.703565
754.656615	108.154738	49.708570
751.313802	100.478646	49.713575
748.227147	94.244458	49.718580
744.311778	90.578932	49.723585
741.171925	91.575543	49.728589
737.237392	79.367697	49.733594
733.576862	89.163799	49.738599
730.386883	89.159429	49.743604
726.718312	99.018726	49.748609
723.212770	92.097916	49.753613
719.765374	92.853004	49.758618
716.362496	99.651096	49.763623
712.958451	82.840213	49.768628
709.303151	87.090633	49.773633
705.991161	92.207989	49.778637
702.375543	93.600174	49.783642
698.937262	87.420929	49.788647
695.209521	87.962070	49.793652
691.262965	95.237287	49.798657
688.153374	80.359425	49.803661
684.812213	89.915357	49.808666
681.495500	93.766548	49.813671
677.920569	91.961651	49.818676
674.022670	92.597401	49.823681
670.918909	89.702076	49.828685
667.259128	93.119211	49.833690
663.949846	97.756567	49.838695
660.603773	94.156699	49.843700
656.700013	99.138388	49.848705
653.456521	84.012338	49.853709
650.020831	93.165395	49.858714
646.261550	86.552619	49.863719
642.827728	90.529915	49.868724
639.099328	97.908829	49.873729
635.818891	88.169553	49.878733
632.041182	93.449986	49.883738
628.704827	94.964693	49.888743
625.364901	93.979329	49.893748
621.812604	93.757033	49.898753
618.142522	95.460149	49.903757
614.608994	106.582207	49.908762
611.068660	92.093101	49.913767
607.793535	93.211365	49.918772
604.349824	93.155633	49.923777
600.966594	87.719514	49.928781
597.574526	93.533838	49.933786
593.501340	101.498819	49.938791
590.419614	92.555172	49.943796
586.243446	105.494194	49.948801
583.227024	91.313206	49.953805
579.651990	95.635381	49.958810
575.975445	93.923684	49.963815
573.003405	91.703665	49.968820
569.390797	86.835436	49.973825
566.030329	87.499688	49.978829
562.355250	87.851269	49.983834
558.502189	83.266742	49.988839
555.008360	84.278397	49.993844
551.598155	89.169248	49.998849
548.199193	87.852224	50.003853
544.809358	81.452662	50.008858
541.141081	84.192505	50.013863
537.685191	91.326575	50.018868
534.225083	99.354390	50.023873
530.904093	90.386762	50.028877
527.114177	83.878176	50.033882
523.586666	83.270235	50.038887
520.126608	83.169596	50.043892
516.279768	90.603646	50.048897
513.076164	85.487254	50.053901
509.909629	83.195704	50.058906
506.240593	79.571528	50.063911
502.961985	73.150564	50.068916
498.634447	86.278585	50.073921
495.309892	91.601936	50.078925
492.227787	87.668114	50.083930
488.719115	89.051233	50.088935
485.092712	82.011430	50.093940
481.659712	87.697998	50.098945
478.367752	87.019307	50.103949
474.768835	84.590536	50.108954
470.996976	85.408029	50.113959
467.899245	76.212965	50.118964
464.112654	93.021039	50.123969
460.475161	74.774081	50.128973
456.825354	91.302658	50.133978
453.578601	87.651378	50.138983
450.363524	85.057797	50.143988
446.836784	90.158158	50.148993
442.941475	86.008263	50.153997
439.476710	87.989612	50.159002
435.918696	89.780174	50.164007
432.605695	84.561338	50.169012
429.144141	85.195397	50.174017
425.602467	82.871049	50.179021
422.020528	91.114574	50.184026
418.249606	90.996182	50.189031
415.445365	85.824429	50.194036
411.744324	81.778906	50.199041
407.892982	81.166414	50.204045
404.306394	84.701229	50.209050
401.096951	93.371780	50.214055
397.706043	79.102723	50.219060
394.229319	79.321692	50.224065
390.528862	74.929901	50.229069
386.785810	83.538248	50.234074
383.043541	88.526259	50.239079
380.071958	79.334773	50.244084
376.617181	83.949035	50.249089
372.863426	75.333486	50.254093
369.455437	76.763174	50.259098
365.948173	76.313181	50.264103
362.827606	81.904583	50.269108
358.914124	101.801304	50.274113
355.557316	84.952974	50.279117
352.165084	79.342980	50.284122
348.571427	75.376047	50.289127
345.271417	81.189777	50.294132
341.612186	93.653918	50.299137
338.122832	91.720437	50.304141
334.480856	89.785140	50.309146
330.439056	92.923421	50.314151
327.536921	76.949874	50.319156
323.912095	88.383786	50.324161
320.573631	75.804891	50.329165
316.925865	91.526963	50.334170
313.500839	89.612959	50.339175
309.964799	73.123601	50.344180
306.211564	85.293697	50.349185
302.962239	76.460390	50.354189
299.730775	79.983846	50.359194
295.930981	84.713355	50.364199
292.674734	71.003021	50.369204
288.615883	93.170976	50.374209
285.276429	92.257141	50.379213
281.806949	95.370747	50.384218
278.113891	93.383642	50.389223
275.068635	80.808127	50.394228
271.267915	83.301847	50.399233
267.783436	75.371447	50.404237
264.369031	86.358432	50.409242
260.794312	87.198132	50.414247
257.737538	77.203420	50.419252
253.802394	88.031282	50.424257
250.277759	76.925848	50.429261
247.058066	69.247984	50.434266
243.683359	83.677945	50.439271
239.992662	81.929914	50.444276
236.372173	100.485873	50.449281
232.805093	86.811528	50.454285
229.374579	79.806907	50.459290
225.756075	82.275480	50.464295
222.524426	85.112354	50.469300
218.860936	94.608873	50.474305
215.645261	99.962509	50.479309
211.824938	81.132197	50.484314
208.085442	79.924403	50.489319
204.951117	82.153659	50.494324
201.294717	84.358878	50.499329
197.782045	88.101988	50.504333
194.525523	78.949892	50.509338
190.993296	87.932830	50.514343
187.587207	82.588437	50.519348
183.357702	74.473774	50.524353
180.031866	83.868049	50.529357
176.882330	88.847222	50.534362
172.939403	85.558355	50.539367
169.799104	75.144098	50.544372
166.302239	79.568597	50.549377
163.027103	84.846936	50.554381
159.487747	80.390785	50.559386
155.672846	88.815287	50.564391
152.081846	70.208882	50.569396
148.983660	67.489207	50.574401
145.728857	86.547594	50.579405
141.816033	80.594488	50.584410
138.225293	92.383738	50.589415
134.890672	82.257817	50.594420
131.268126	88.164995	50.599425
127.566437	89.226120	50.604429
124.354364	90.157215	50.609434
120.782498	90.200856	50.614439
117.116081	87.669697	50.619444
113.655334	93.950794	50.624449
110.353317	88.492960	50.629453
106.988560	81.114690	50.634458
103.317545	84.409178	50.639463
100.080490	74.714175	50.644468
96.302148	87.579409	50.649473
92.762203	85.181962	50.654477
89.101486	83.241028	50.659482
85.518774	84.247298	50.664487
82.556649	77.428587	50.669492
78.807904	85.315665	50.674497
75.336483	77.992333	50.679501
71.628515	88.194361	50.684506
67.746890	84.193888	50.689511
64.568850	83.177631	50.694516
60.810445	78.851954	50.699521
57.774738	74.678657	50.704525
54.321301	79.074923	50.709530
50.817247	84.611442	50.714535
48.039104	81.841100	50.719540
43.675621	84.757063	50.724545
39.970015	86.052011	50.729549
36.635781	75.103496	50.734554
32.970360	70.013476	50.739559
29.989478	70.995203	50.744564
25.901897	93.876168	50.749569
22.684019	85.796497	50.754573
19.089551	85.056060	50.759578
15.243309	73.011549	50.764583
12.474703	71.683782	50.769588
8.483832	78.894562	50.774593
5.398909	74.769381	50.779597
1.327904	85.248083	50.784602