Thu Jun 16 18:16:14 2022

Number of Points = 9928

Depth (nm)	Load (N)	Time (s)
1.178717	132.309660	0.000000
1.194624	108.264343	0.005005
0.993282	101.794808	0.010010
0.860007	104.137228	0.015014
0.895094	87.068787	0.020019
0.241816	72.970798	0.025024
0.560970	64.974101	0.030029
-0.300040	57.544958	0.035034
-0.719094	42.570210	0.040038
-0.420485	36.678288	0.045043
-0.822348	30.738749	0.050048
-0.718361	22.174156	0.055053
-1.693867	11.553114	0.060058
-2.096321	10.340856	0.065062
-1.854930	-0.710351	0.070067
-2.652691	1.929406	0.075072
-2.957131	-15.116158	0.080077
-3.051140	-9.757546	0.085082
-3.450610	-6.874424	0.090086
-3.049331	-17.807313	0.095091
-4.143530	-11.215473	0.100096
-4.732771	-8.138013	0.105101
-4.885490	-12.365305	0.110106
-5.213029	-6.843696	0.115110
-5.040787	-14.225819	0.120115
-5.088761	-9.091461	0.125120
-4.708885	-14.708918	0.130125
-5.011984	-1.570225	0.135130
-6.233546	-5.130178	0.140134
-6.061735	-9.627550	0.145139
-6.344965	-7.136850	0.150144
-6.957797	-16.139480	0.155149
-7.422039	-9.500109	0.160154
-7.434833	-9.513478	0.165158
-7.465824	-8.743476	0.170163
-8.096711	0.049657	0.175168
-8.048214	-9.593325	0.180173
-8.000315	-12.271537	0.185178
-8.228685	-9.981689	0.190182
-8.226761	-9.332553	0.195187
-9.161187	-6.866340	0.200192
-9.736343	-3.098547	0.205197
-9.700081	-2.815868	0.210202
-9.480888	-4.167160	0.215206
-9.390555	-6.721666	0.220211
-10.319943	-10.922719	0.225216
-10.848278	-6.975121	0.230221
-10.796692	-5.034605	0.235226
-11.293107	-8.947906	0.240230
-11.412654	-8.576044	0.245235
-11.647993	-3.693073	0.250240
-11.485563	-5.146958	0.255245
-11.333114	-3.914882	0.260250
-12.393965	-4.079926	0.265254
-12.449943	-11.688830	0.270259
-13.070830	-8.134272	0.275264
-12.723290	-7.516304	0.280269
-12.973026	-13.024979	0.285274
-13.623371	-9.798908	0.290278
-13.914574	-7.007077	0.295283
-14.639299	-3.009759	0.300288
-14.908795	-2.490191	0.305293
-14.685120	-2.671679	0.310298
-14.570034	-5.424233	0.315302
-14.317041	-15.902579	0.320307
-14.728465	-7.623998	0.325312
-15.116291	5.082285	0.330317
-15.610920	-8.213730	0.335322
-16.028571	-8.672017	0.340326
-15.963648	-19.926675	0.345331
-16.471799	-7.310518	0.350336
-17.069415	-16.670227	0.355341
-17.400389	-2.081532	0.360346
-17.963811	-4.887601	0.365350
-17.766345	-15.111218	0.370355
-17.908359	-0.781642	0.375360
-18.016004	-3.767704	0.380365
-17.889466	-3.784465	0.385370
-18.170108	-10.604884	0.390374
-18.222999	-21.932807	0.395379
-19.113983	-15.048199	0.400384
-19.212677	-13.736836	0.405389
-19.463143	-10.470694	0.410394
-19.473471	-10.711575	0.415398
-19.970297	-8.860576	0.420403
-20.844469	-10.215668	0.425408
-20.987680	-7.461020	0.430413
-20.904594	-10.523488	0.435418
-21.207908	-9.771919	0.440422
-21.079352	-19.228248	0.445427
-21.060483	-12.045806	0.450432
-21.253289	-12.274684	0.455437
-21.877560	-25.225866	0.460442
-22.341340	-23.051710	0.465446
-22.253671	-14.883334	0.470451
-22.523876	-4.024479	0.475456
-22.977917	-11.180970	0.480461
-23.520119	-17.412893	0.485466
-24.188618	-17.548163	0.490470
-23.863158	-13.167389	0.495475
-24.077398	-17.904721	0.500480
-23.752123	-13.561899	0.505485
-23.691230	-12.018727	0.510490
-24.650626	-2.837853	0.515494
-24.988115	-16.621534	0.520499
-25.399246	-12.891800	0.525504
-25.364835	-12.359217	0.530509
-25.502385	-20.408450	0.535514
-25.972860	-14.770783	0.540518
-26.758361	-9.169251	0.545523
-27.005376	-4.738067	0.550528
-26.905668	-3.972695	0.555533
-26.866592	-9.552578	0.560538
-27.093958	-10.337980	0.565542
-27.159126	-26.017625	0.570547
-27.964760	-9.990634	0.575552
-28.435421	-7.887554	0.580557
-28.412713	-18.003660	0.585562
-29.138206	-14.979647	0.590566
-28.825111	-20.576002	0.595571
-29.028084	-7.616941	0.600576
-28.941270	-15.377889	0.605581
-29.180357	-21.678251	0.610586
-29.876384	-6.535958	0.615590
-29.702346	-18.590885	0.620595
-30.524602	-7.970706	0.625600
-30.558987	-7.791286	0.630605
-30.140788	-20.223962	0.635610
-31.399930	-14.712958	0.640614
-31.559802	-12.210680	0.645619
-32.138051	-0.769362	0.650624
-32.235407	-1.793489	0.655629
-32.109173	-8.700286	0.660634
-32.269688	-10.643702	0.665638
-32.325130	-17.778158	0.670643
-32.250093	-6.102373	0.675648
-32.593738	-18.187274	0.680653
-33.349707	-14.874887	0.685658
-33.725282	0.696683	0.690662
-33.640055	-12.314341	0.695667
-33.852073	-14.658960	0.700672
-34.125497	-17.708188	0.705677
-34.876381	-18.263037	0.710682
-35.383977	-3.213047	0.715686
-35.080271	-9.587823	0.720691
-35.800842	-4.731508	0.725696
-35.375217	-0.056618	0.730701
-35.449684	-8.974780	0.735706
-35.532928	-8.737563	0.740710
-36.273811	-12.321104	0.745715
-37.061705	-7.802706	0.750720
-36.780262	-11.697949	0.755725
-36.747213	-15.482985	0.760730
-37.042483	-11.250609	0.765734
-37.231719	-20.686087	0.770739
-37.849708	-16.280909	0.775744
-38.683529	-14.543413	0.780749
-38.352906	-14.840145	0.785754
-38.729769	-11.328675	0.790758
-38.330981	-27.541861	0.795763
-38.628422	-19.059657	0.800768
-39.223914	-21.312292	0.805773
-39.937098	-13.590872	0.810778
-39.995846	-25.916607	0.815782
-40.121622	-20.220381	0.820787
-40.238546	-15.183843	0.825792
-39.946999	-16.540778	0.830797
-40.650229	-23.896897	0.835802
-41.649944	-21.392466	0.840806
-41.174663	-20.557063	0.845811
-41.962519	-18.292550	0.850816
-42.200973	-26.161730	0.855821
-41.638273	-22.591847	0.860826
-42.180734	-24.510616	0.865830
-43.055522	-29.538433	0.870835
-43.233074	-20.637027	0.875840
-43.492890	-22.919288	0.880845
-43.657052	-20.594177	0.885850
-43.614141	-17.004393	0.890854
-43.343608	-20.965706	0.895859
-43.632808	-21.450349	0.900864
-43.689028	-12.414298	0.905869
-44.187148	-22.523351	0.910874
-44.821339	-14.255512	0.915878
-45.213473	-15.960478	0.920883
-45.320932	-13.780487	0.925888
-45.627690	-18.264669	0.930893
-46.168346	-24.812341	0.935898
-46.720368	-19.236965	0.940902
-46.531171	-20.169934	0.945907
-46.609771	-20.585398	0.950912
-47.077247	-19.082372	0.955917
-46.765165	-21.282157	0.960922
-47.080824	-16.739399	0.965926
-46.935642	-8.691613	0.970931
-47.852231	-14.430834	0.975936
-48.343569	-9.927409	0.980941
-48.273063	-15.311029	0.985946
-48.466096	-19.291527	0.990950
-48.335894	-26.171348	0.995955
-49.238100	-16.706432	1.000960
-49.858991	-11.664645	1.005965
-49.621471	-22.052821	1.010970
-49.801893	-14.850174	1.015974
-49.679567	-17.131166	1.020979
-50.235449	-13.979701	1.025984
-50.298230	-15.723212	1.030989
-50.471734	-14.220328	1.035994
-51.010916	-12.137690	1.040998
-51.319154	-13.405370	1.046003
-51.326064	-12.763160	1.051008
-52.084486	-18.040076	1.056013
-52.394679	-18.575510	1.061018
-53.018284	-13.548664	1.066022
-52.510008	-25.452039	1.071027
-52.932050	-25.492977	1.076032
-52.764924	-21.688035	1.081037
-52.673028	-18.355451	1.086042
-53.578694	-12.860635	1.091046
-54.221626	-19.669712	1.096051
-54.266958	-11.503922	1.101056
-54.601104	-15.592411	1.106061
-54.276974	-17.258490	1.111066
-54.445133	-12.050704	1.116070
-54.987641	-21.167741	1.121075
-55.685986	-5.540866	1.126080
-55.976964	-10.313462	1.131085
-55.890933	-17.544104	1.136090
-56.169263	-10.873503	1.141094
-56.282967	-18.349739	1.146099
-56.536124	-16.022647	1.151104
-56.485744	-9.090572	1.156109
-57.208052	-9.432409	1.161114
-57.827849	-8.551486	1.166118
-57.745765	-20.643697	1.171123
-57.670091	-13.778352	1.176128
-58.046558	-17.497387	1.181133
-58.163259	-7.677390	1.186138
-58.576303	0.029754	1.191142
-58.873172	-14.936901	1.196147
-59.374508	-10.857521	1.201152
-59.392059	-16.090147	1.206157
-59.329512	-23.448709	1.211162
-59.650662	-3.217186	1.216166
-60.147630	-13.084727	1.221171
-60.807747	-21.872845	1.226176
-61.215174	-16.927700	1.231181
-60.879749	-23.610484	1.236186
-60.937904	-12.592035	1.241190
-61.099469	-12.264331	1.246195
-61.120371	-19.432116	1.251200
-61.758809	-22.166488	1.256205
-62.349595	-16.760607	1.261210
-62.755248	-11.308073	1.266214
-62.974702	-20.501485	1.271219
-62.668818	-23.556967	1.276224
-62.967940	-20.434321	1.281229
-62.948550	-22.658839	1.286234
-63.748004	-14.142306	1.291238
-64.272272	-16.101766	1.296243
-63.968922	-13.089241	1.301248
-64.413189	-19.262068	1.306253
-64.098216	-19.195828	1.311258
-64.684193	-27.120137	1.316262
-65.483043	-18.231974	1.321267
-65.900969	-14.894355	1.326272
-66.223470	-10.450500	1.331277
-65.729119	-12.155662	1.336282
-66.347725	-13.988151	1.341286
-66.287500	-17.833416	1.346291
-66.141224	-18.800432	1.351296
-66.685534	-9.190837	1.356301
-67.050416	-21.823110	1.361306
-67.859215	-15.058135	1.366310
-67.589805	-20.565584	1.371315
-67.645425	-17.847118	1.376320
-67.835626	-13.652035	1.381325
-68.313040	-11.984387	1.386330
-69.029020	-6.853383	1.391334
-69.405086	-14.645563	1.396339
-69.404229	-3.456125	1.401344
-69.343432	-9.444378	1.406349
-69.111496	-15.556607	1.411354
-69.596732	-20.204951	1.416358
-69.835320	-17.606202	1.421363
-70.107138	-2.277806	1.426368
-70.869237	-4.084805	1.431373
-70.955931	-10.070880	1.436378
-71.439003	-12.569294	1.441382
-71.325349	-20.860998	1.446387
-70.986414	-8.983773	1.451392
-72.331871	-18.229449	1.456397
-72.328460	-16.646689	1.461402
-72.837290	1.399269	1.466406
-72.797944	-7.792229	1.471411
-72.797736	-14.427510	1.476416
-73.044763	-12.425118	1.481421
-72.916310	-14.769276	1.486426
-73.751758	-5.520095	1.491430
-74.404570	-10.628301	1.496435
-74.305358	-13.299700	1.501440
-74.464831	-4.964103	1.506445
-74.513072	-12.786093	1.511450
-75.000831	-4.979294	1.516454
-74.611958	-22.235208	1.521459
-75.511227	-21.152024	1.526464
-75.860397	-9.424984	1.531469
-75.744764	-16.575970	1.536474
-76.416460	-5.492919	1.541478
-75.937826	-17.538002	1.546483
-76.445044	2.862491	1.551488
-77.256781	-1.153088	1.556493
-77.189224	-8.461873	1.561498
-77.768220	-11.591119	1.566502
-77.897043	-18.450923	1.571507
-77.828423	-13.343731	1.576512
-77.719504	-5.861069	1.581517
-77.791976	-16.813821	1.586522
-78.524380	-5.862407	1.591526
-78.920313	-8.384989	1.596531
-79.194318	-17.134514	1.601536
-79.194604	-16.007621	1.606541
-80.075602	-19.299556	1.611546
-80.207748	-12.196145	1.616550
-80.317129	-11.214200	1.621555
-80.789226	-16.912434	1.626560
-80.740533	-12.535154	1.631565
-80.544556	-17.741210	1.636570
-80.805186	-9.457069	1.641574
-81.045246	-14.486688	1.646579
-81.881528	-15.067472	1.651584
-82.390702	-14.946025	1.656589
-82.359620	-26.282092	1.661594
-82.884034	-11.355613	1.666598
-82.523250	-21.144111	1.671603
-82.525885	-17.734246	1.676608
-82.688960	-21.461117	1.681613
-83.076643	-16.705002	1.686618
-84.241550	-14.709652	1.691622
-83.956310	-13.319873	1.696627
-84.481367	-22.593099	1.701632
-84.341834	-14.007308	1.706637
-84.125482	-13.433368	1.711642
-84.998219	-5.296182	1.716646
-85.558491	-8.065274	1.721651
-85.442607	-0.305257	1.726656
-85.772748	-1.760115	1.731661
-85.771666	-11.313270	1.736666
-85.828926	-11.519658	1.741670
-85.877612	-8.780337	1.746675
-86.717825	-15.799892	1.751680
-87.143376	-2.424620	1.756685
-87.075522	-14.331968	1.761690
-87.091846	-16.636513	1.766694
-87.804647	-16.518310	1.771699
-88.286807	-15.862472	1.776704
-88.941317	-9.068633	1.781709
-88.446813	-14.930559	1.786714
-88.889396	-13.992400	1.791718
-88.703096	-18.576218	1.796723
-88.710264	-17.860665	1.801728
-89.246178	-18.947171	1.806733
-89.373256	-16.325219	1.811738
-89.934251	-9.689195	1.816742
-90.133599	-19.008161	1.821747
-90.311008	-18.856206	1.826752
-90.771622	-13.858861	1.831757
-90.905262	-11.811476	1.836762
-91.877033	-11.346616	1.841766
-92.046122	-11.686057	1.846771
-91.992442	-18.695985	1.851776
-92.278807	-8.046280	1.856781
-92.108539	-18.307717	1.861786
-91.989402	-8.471651	1.866790
-92.262199	-10.730751	1.871795
-92.466061	-5.237671	1.876800
-93.333729	-11.408102	1.881805
-93.412562	-18.449010	1.886810
-93.646178	-10.265227	1.891814
-93.363940	-20.608109	1.896819
-94.108366	-12.056274	1.901824
-94.993307	-16.584790	1.906829
-95.155408	-26.868834	1.911834
-95.428525	-15.566846	1.916838
-95.437166	-14.849669	1.921843
-95.302347	-23.678690	1.926848
-95.388163	-21.093944	1.931853
-95.388883	-13.252708	1.936858
-96.332844	-15.681658	1.941862
-96.504059	-7.692277	1.946867
-96.768498	-14.635426	1.951872
-96.986394	-11.456354	1.956877
-97.136636	-26.318675	1.961882
-97.067621	-10.668869	1.966886
-97.590561	-14.161746	1.971891
-97.960138	-13.199938	1.976896
-98.617227	-10.728249	1.981901
-98.630571	-22.328080	1.986906
-98.940924	-18.663440	1.991910
-98.678888	-13.073728	1.996915
-98.791948	-21.611837	2.006912
-98.992631	-17.426874	2.016909
-98.886955	-11.478222	2.026906
-97.993115	-10.595346	2.036902
-97.472440	-6.314847	2.046899
-97.085722	-1.723666	2.056896
-96.124007	-3.456087	2.066893
-95.763921	-5.422563	2.076890
-95.674403	-10.414551	2.086886
-94.953119	-3.056278	2.096883
-94.371055	-2.732937	2.106880
-93.985664	-8.247877	2.116877
-92.937258	-8.215667	2.126874
-92.720368	-13.104635	2.136870
-92.567545	-9.009407	2.146867
-92.445802	-13.035104	2.156864
-91.304187	-16.977263	2.166861
-90.930712	-14.639769	2.176858
-90.240501	-16.981447	2.186854
-89.608074	-12.193406	2.196851
-89.435547	-10.498664	2.206848
-89.328482	-11.751708	2.216845
-88.475622	-10.617376	2.226842
-88.327994	-9.175251	2.236838
-87.144181	-4.561310	2.246835
-86.708189	-11.716581	2.256832
-86.329928	-8.636348	2.266829
-86.204572	-10.469102	2.276826
-85.486500	-12.863590	2.286822
-85.158051	-1.969507	2.296819
-83.613097	-4.470721	2.306816
-83.787235	-2.870216	2.316813
-83.432476	-9.173704	2.326810
-83.305924	-14.731310	2.336806
-82.307232	-10.767972	2.346803
-81.946684	-12.432054	2.356800
-81.499431	-11.094370	2.366797
-80.796148	-5.733249	2.376794
-80.694390	-8.191440	2.386790
-79.636629	-12.950788	2.396787
-78.837808	-7.105820	2.406784
-78.613549	-10.045862	2.416781
-78.625618	-10.479679	2.426778
-78.239958	-8.686310	2.436774
-77.491495	-6.965050	2.446771
-77.186476	-7.146629	2.456768
-75.977540	-2.494459	2.466765
-75.802816	-12.726567	2.476762
-75.495638	-6.599820	2.486758
-75.061085	-8.336982	2.496755
-74.332074	-10.315431	2.506752
-74.023401	-11.237586	2.516749
-72.904434	-15.146167	2.526746
-72.374904	-13.310688	2.536742
-72.461849	-12.331903	2.546739
-72.428457	-6.636431	2.556736
-71.427931	-6.629099	2.566733
-71.187538	-11.657382	2.576730
-70.053876	-9.074790	2.586726
-69.517671	-6.806071	2.596723
-69.506631	-9.377290	2.606720
-69.306825	-8.444412	2.616717
-68.354419	-9.235778	2.626714
-67.987226	-10.708334	2.636710
-66.794552	-11.958439	2.646707
-66.725386	-7.476779	2.656704
-66.213017	-12.488666	2.666701
-66.001353	-19.302415	2.676698
-65.747922	-8.321652	2.686694
-64.883149	-9.413253	2.696691
-64.398289	-7.209245	2.706688
-63.381179	-11.188611	2.716685
-63.360231	-19.833072	2.726682
-63.190602	-9.557194	2.736678
-62.058000	-7.840443	2.746675
-61.634418	-9.819485	2.756672
-61.359539	-12.492489	2.766669
-61.278865	-17.461875	2.776666
-60.175239	-4.701302	2.786662
-59.922895	-7.382238	2.796659
-59.004055	-13.097551	2.806656
-58.563437	-14.381121	2.816653
-58.223885	-14.163204	2.826650
-58.215948	-16.500094	2.836646
-57.767653	-10.579117	2.846643
-56.784325	-12.792514	2.856640
-56.149193	-16.377735	2.866637
-55.413185	-13.510920	2.876634
-55.292914	-10.478336	2.886630
-55.325262	-23.284050	2.896627
-54.265039	-8.864876	2.906624
-53.803633	-17.365403	2.916621
-53.384395	-12.731390	2.926618
-52.430975	-13.324864	2.936614
-52.282709	-17.269697	2.946611
-52.455455	-13.359220	2.956608
-51.566118	-16.448389	2.966605
-50.867669	-11.870396	2.976602
-49.959853	-12.298678	2.986598
-49.620447	-16.300979	2.996595
-49.508742	-14.010410	3.006592
-48.818335	-13.195553	3.016589
-48.097425	-13.261238	3.026586
-47.763943	-17.220677	3.036582
-47.488059	-15.634979	3.046579
-46.482540	-17.220037	3.056576
-45.962346	-18.351496	3.066573
-46.134843	-12.912022	3.076570
-45.422909	-13.086858	3.086566
-44.419781	-15.181036	3.096563
-44.461840	-15.191953	3.106560
-44.200838	-14.673402	3.116557
-43.217664	-18.766286	3.126554
-42.931281	-11.368339	3.136550
-42.038239	-14.887523	3.146547
-41.527400	-12.677137	3.156544
-41.139688	-22.163967	3.166541
-41.089640	-10.725620	3.176538
-40.396300	-13.344104	3.186534
-39.821031	-16.803561	3.196531
-39.336319	-10.433414	3.206528
-38.409128	-14.582836	3.216525
-38.233899	-19.136075	3.226522
-38.061262	-15.932165	3.236518
-37.185310	-16.184781	3.246515
-36.703507	-14.334200	3.256512
-36.352045	-8.468241	3.266509
-35.832215	-16.023403	3.276506
-35.210293	-17.033873	3.286502
-35.121382	-17.225175	3.296499
-33.906580	-21.635789	3.306496
-33.597869	-9.093136	3.316493
-33.265091	-21.202429	3.326490
-33.137692	-8.511768	3.336486
-31.977130	-14.047532	3.346483
-31.640743	-14.059350	3.356480
-31.449550	-12.141085	3.366477
-30.522312	-16.295255	3.376474
-30.157059	-11.190218	3.386470
-29.896429	-23.163912	3.396467
-29.085203	-13.400744	3.406464
-28.396263	-16.940526	3.416461
-28.454272	-14.502285	3.426458
-28.044673	-17.196464	3.436454
-27.912749	-11.993499	3.446451
-26.411144	-12.823264	3.456448
-26.098050	-15.519968	3.466445
-25.910830	-12.681093	3.476442
-25.209124	-16.385184	3.486438
-24.405249	-8.540122	3.496435
-24.347924	-12.590046	3.506432
-24.134816	-11.296244	3.516429
-23.049818	-16.232756	3.526426
-22.645295	-12.173093	3.536422
-22.174091	-18.146925	3.546419
-21.961165	-11.464955	3.556416
-21.169381	-12.097106	3.566413
-20.873847	-16.908290	3.576410
-20.036872	-21.187416	3.586406
-19.554606	-18.368358	3.596403
-19.419306	-13.800030	3.606400
-18.904551	-19.653235	3.616397
-17.992196	-22.544391	3.626394
-17.664029	-17.403690	3.636390
-17.500174	-24.487313	3.646387
-16.368723	-18.958287	3.656384
-16.150604	-12.789455	3.666381
-16.053707	-16.444568	3.676378
-15.247460	-20.109233	3.686374
-14.544496	-13.838965	3.696371
-14.432670	-10.735934	3.706368
-13.588756	-15.582029	3.716365
-13.316050	-10.691066	3.726362
-12.986525	-12.702077	3.736358
-11.841151	-11.618147	3.746355
-11.590815	-18.490743	3.756352
-11.551517	-19.169236	3.766349
-10.229258	-11.470589	3.776346
-9.774340	-9.002424	3.786342
-9.935617	-16.786518	3.796339
-9.794245	-14.062358	3.806336
-8.795929	-22.590760	3.816333
-8.270235	-20.701201	3.826330
-7.074511	-17.623487	3.836326
-7.105777	-17.716003	3.846323
-6.964559	-13.797054	3.856320
-6.471256	-11.039185	3.866317
-5.564331	-12.623946	3.876314
-5.256225	-14.730495	3.886310
-4.654386	-10.364319	3.896307
-3.971223	-2.124129	3.906304
-3.872190	-10.921675	3.916301
-3.596905	0.303138	3.926298
-3.205101	-0.562518	3.936294
-2.494746	22.048894	3.946291
-2.049195	36.827427	3.956288
-1.537031	49.988177	3.966285
-1.249606	64.860039	3.976282
-1.056691	89.449231	3.986278
-0.478850	105.609961	3.996275
0.000000	130.786199	4.001280
-0.089496	130.581287	4.006285
0.339390	154.054243	4.011290
0.422690	158.018505	4.016294
0.721433	166.277688	4.021299
0.469918	168.856109	4.026304
0.429380	195.889670	4.031309
1.059842	198.107867	4.036314
0.671617	194.779721	4.041318
0.894924	199.653458	4.046323
1.101641	200.961330	4.051328
0.947696	209.744331	4.056333
0.913749	205.104105	4.061338
1.097704	204.860613	4.066342
1.341728	208.005721	4.071347
0.603509	207.152893	4.076352
1.034125	215.889415	4.081357
1.532428	222.532013	4.086362
1.685524	230.456781	4.091366
1.467800	211.173502	4.096371
1.383688	209.826636	4.101376
1.391350	212.945098	4.106381
1.297268	201.828034	4.111386
1.205107	206.296829	4.116390
1.579937	201.969374	4.121395
1.412650	209.599607	4.126400
1.188893	206.793600	4.131405
1.613992	203.480118	4.136410
1.398521	208.849900	4.141414
1.399898	198.526542	4.146419
1.496078	200.518119	4.151424
1.360008	205.499983	4.156429
1.632905	201.575120	4.161434
1.190932	202.183277	4.166438
1.386195	205.855968	4.171443
1.509311	204.985898	4.176448
1.601912	207.615686	4.181453
1.607501	204.944330	4.186458
1.563844	215.973970	4.191462
1.250611	206.497672	4.196467
1.395019	203.346102	4.201472
1.336613	197.175414	4.206477
1.680867	194.206978	4.211482
1.513394	203.712503	4.216486
1.591699	200.575606	4.221491
1.912846	206.146761	4.226496
1.591309	198.727055	4.231501
1.900773	197.443207	4.236506
1.504364	211.295792	4.241510
1.508519	206.332877	4.246515
1.520243	206.803906	4.251520
1.371355	195.167794	4.256525
1.756000	201.800753	4.261530
1.345701	205.126204	4.266534
1.508508	206.947146	4.271539
1.326333	203.011160	4.276544
1.227001	203.355614	4.281549
1.595178	202.411209	4.286554
1.252694	225.772997	4.291558
1.621598	227.234414	4.296563
1.794723	235.108914	4.301568
1.313985	234.493523	4.306573
2.080552	229.506818	4.311578
1.683275	237.658095	4.316582
1.602162	237.507242	4.321587
1.993090	234.623131	4.326592
1.907525	237.071043	4.331597
1.969899	228.731243	4.336602
2.089847	241.591969	4.341606
2.190172	233.796301	4.346611
2.187952	233.706502	4.351616
1.799981	229.990979	4.356621
2.067788	229.632211	4.361626
1.922078	239.332857	4.366630
1.800787	219.369967	4.371635
1.627489	217.609767	4.376640
1.800890	228.254598	4.381645
1.946939	228.996539	4.386650
1.696635	237.710437	4.391654
1.854536	243.456864	4.396659
2.031687	246.507467	4.401664
1.907123	241.390597	4.406669
2.230911	232.755527	4.411674
2.028287	231.097250	4.416678
2.101404	233.270324	4.421683
2.391984	242.738654	4.426688
1.945498	232.003004	4.431693
1.909485	228.580242	4.436698
1.768747	236.167723	4.441702
1.964712	235.907941	4.446707
1.908266	238.567495	4.451712
1.973399	244.863578	4.456717
2.258571	235.099149	4.461722
1.921854	243.661686	4.466726
1.628014	226.487919	4.471731
1.988046	239.479349	4.476736
1.879900	263.066671	4.481741
2.569034	264.099980	4.486746
2.233155	271.392678	4.491750
2.566015	261.770606	4.496755
2.258641	251.068583	4.501760
2.169936	257.636144	4.506765
2.222148	245.238871	4.511770
2.300598	257.828255	4.516774
2.338312	261.657024	4.521779
2.170495	252.230068	4.526784
2.125712	258.904023	4.531789
2.392910	264.892456	4.536794
2.267607	274.288353	4.541798
2.425484	275.288600	4.546803
2.463822	265.734632	4.551808
2.298321	269.381124	4.556813
2.173288	266.248909	4.561818
2.289842	271.177109	4.566822
2.020855	268.968929	4.571827
2.241289	266.398501	4.576832
2.192842	283.090517	4.581837
2.282773	273.819846	4.586842
2.461402	269.848884	4.591846
2.303186	275.213963	4.596851
2.290595	272.022420	4.601856
2.261144	278.430436	4.606861
2.661236	277.291035	4.611866
2.408971	270.157003	4.616870
2.506080	274.249438	4.621875
3.068916	288.686166	4.626880
2.112755	286.035016	4.631885
2.292133	286.349199	4.636890
2.144230	306.388934	4.641894
2.567511	308.066016	4.646899
2.454998	313.391788	4.651904
2.574151	313.425478	4.656909
3.217696	303.487440	4.661914
2.791916	301.241729	4.666918
2.598112	307.586349	4.671923
3.103589	304.961806	4.676928
3.067150	311.433046	4.681933
2.535284	287.816660	4.686938
2.490427	291.733568	4.691942
2.872221	305.879693	4.696947
2.676377	302.876772	4.701952
2.947576	307.587738	4.706957
3.035253	308.431475	4.711962
2.651753	291.877616	4.716966
2.481984	296.249555	4.721971
2.791376	288.698609	4.726976
3.059363	298.276666	4.731981
3.021443	306.034146	4.736986
2.728975	302.087454	4.741990
3.082323	295.550049	4.746995
3.068743	286.201469	4.752000
2.685086	288.702497	4.757005
3.106175	287.324526	4.762010
3.037831	285.047670	4.767014
2.647961	283.568513	4.772019
2.801476	284.480689	4.777024
2.638224	303.216637	4.782029
3.085884	303.358725	4.787034
3.118798	300.745879	4.792038
2.423529	293.807180	4.797043
2.720092	294.850216	4.802048
2.257015	302.553052	4.807053
2.471076	298.475893	4.812058
2.487605	305.381743	4.817062
2.647619	326.106504	4.822067
2.817647	336.762031	4.827072
2.866990	341.150654	4.832077
3.035961	338.417351	4.837082
3.118148	329.719055	4.842086
3.314930	340.024664	4.847091
3.371246	351.069057	4.852096
2.707182	346.282030	4.857101
3.044760	348.647702	4.862106
3.163519	347.684325	4.867110
2.856609	354.456098	4.872115
3.081601	340.834958	4.877120
3.035102	349.472620	4.882125
3.220559	341.853634	4.887130
2.965828	344.833066	4.892134
2.848343	346.211889	4.897139
2.975203	352.108710	4.902144
3.164167	370.113788	4.907149
3.366604	379.823485	4.912154
3.439544	372.377970	4.917158
3.424960	372.524624	4.922163
3.425796	378.011343	4.927168
3.222307	378.298921	4.932173
3.577777	374.608099	4.937178
3.383565	379.018335	4.942182
3.603955	377.154779	4.947187
3.492069	363.988360	4.952192
3.533514	358.337213	4.957197
3.563673	352.246145	4.962202
3.310996	352.749229	4.967206
3.410808	347.007444	4.972211
3.575604	350.282089	4.977216
3.251942	358.196029	4.982221
3.455708	351.222390	4.987226
3.163156	351.866435	4.992230
3.301140	354.623811	4.997235
3.386414	366.762278	5.002240
3.191069	377.354396	5.007245
3.363453	371.365804	5.012250
3.527309	380.530183	5.017254
3.318898	375.199126	5.022259
3.693909	366.777200	5.027264
3.527821	369.398364	5.032269
3.591612	371.987953	5.037274
3.390969	375.616796	5.042278
3.505040	386.222706	5.047283
3.849021	372.510841	5.052288
3.394068	385.442027	5.057293
3.820036	376.355305	5.062298
3.875484	371.811542	5.067302
3.522506	373.114051	5.072307
3.880094	375.783345	5.077312
3.561535	380.747770	5.082317
3.941078	374.709058	5.087322
4.093835	379.641374	5.092326
3.842789	380.225385	5.097331
4.241038	374.548518	5.102336
3.672916	389.592912	5.107341
3.831971	370.312678	5.112346
4.055375	382.062015	5.117350
3.735527	375.903580	5.122355
4.033891	377.729962	5.127360
3.661735	373.964829	5.132365
4.006418	361.103980	5.137370
3.980227	363.847840	5.142374
3.777853	357.660331	5.147379
3.750171	355.647264	5.152384
3.720935	368.106252	5.157389
4.161888	360.873998	5.162394
3.736860	373.432038	5.167398
3.661341	375.327604	5.172403
4.104757	378.078019	5.177408
3.654225	383.351742	5.182413
3.627804	385.486531	5.187418
3.917577	394.908129	5.192422
3.912142	383.105213	5.197427
4.135308	380.226207	5.202432
3.814032	388.351487	5.207437
4.107165	384.707566	5.212442
3.706837	386.630369	5.217446
4.048891	386.684446	5.222451
4.067780	385.866712	5.227456
3.964296	384.528261	5.232461
4.209478	374.761868	5.237466
3.997182	384.565952	5.242470
3.734495	390.348590	5.247475
4.024452	387.052667	5.252480
3.720329	386.728721	5.257485
4.145751	401.752883	5.262490
4.051980	411.529801	5.267494
4.066489	420.219576	5.272499
4.001378	414.639095	5.277504
3.984054	420.212295	5.282509
4.056713	417.021039	5.287514
4.107700	420.512513	5.292518
4.152265	417.789494	5.297523
4.221346	413.959229	5.302528
3.978604	421.734040	5.307533
4.226100	419.306313	5.312538
4.214409	420.810024	5.317542
3.793686	417.595229	5.322547
3.810470	414.545606	5.327552
3.991405	435.468517	5.332557
4.241026	438.112452	5.337562
4.408314	442.716617	5.342566
4.225457	452.565011	5.347571
4.390772	445.487088	5.352576
4.195072	457.891968	5.357581
4.622530	458.989746	5.362586
4.518872	451.534307	5.367590
4.279745	451.918048	5.372595
4.381356	450.785635	5.377600
4.396991	451.710248	5.382605
4.318263	458.787196	5.387610
4.708199	458.690306	5.392614
4.705204	449.889996	5.397619
4.734165	451.672608	5.402624
4.437783	443.444660	5.407629
4.651190	450.887891	5.412634
4.167305	453.752588	5.417638
4.527352	450.464504	5.422643
4.560565	446.442448	5.427648
4.547262	457.086720	5.432653
4.578956	446.755226	5.437658
4.433887	450.696035	5.442662
4.467775	452.667750	5.447667
4.509418	446.717505	5.452672
4.586824	448.134277	5.457677
4.576636	447.361204	5.462682
4.550492	450.352310	5.467686
4.343629	448.732593	5.472691
4.721940	449.028607	5.477696
4.068586	453.200709	5.482701
4.217526	467.744580	5.487706
4.789565	481.323221	5.492710
4.619089	485.169283	5.497715
4.876810	477.775265	5.502720
4.613661	489.996960	5.507725
4.448676	480.100964	5.512730
4.895460	489.871181	5.517734
4.909780	490.874250	5.522739
4.965037	485.664737	5.527744
4.566583	490.804890	5.532749
5.192164	492.469577	5.537754
4.879723	486.885151	5.542758
4.697367	495.974510	5.547763
4.818597	484.571759	5.552768
4.556363	494.449970	5.557773
4.422918	495.450425	5.562778
4.535460	495.296079	5.567782
4.756712	491.492050	5.572787
4.976944	486.362714	5.577792
4.798149	494.200691	5.582797
5.062460	502.656947	5.587802
4.620082	493.339539	5.592806
4.599182	502.418303	5.597811
4.934202	506.753253	5.602816
4.848341	506.138302	5.607821
5.014705	506.722203	5.612826
5.038748	513.405022	5.617830
4.723559	512.622856	5.622835
4.887049	506.079542	5.627840
4.921671	520.333947	5.632845
4.718035	518.609112	5.637850
4.875634	510.784700	5.642854
5.056357	510.023386	5.647859
5.215394	506.081351	5.652864
4.916464	516.064200	5.657869
5.332285	532.883692	5.662874
5.283018	525.938963	5.667878
4.950303	523.963358	5.672883
5.301364	521.218084	5.677888
5.218762	526.828649	5.682893
5.067672	511.825637	5.687898
5.158317	526.032904	5.692902
5.344076	537.735601	5.697907
5.434576	542.275828	5.702912
5.473962	526.669005	5.707917
5.258514	512.222802	5.712922
5.257684	512.579005	5.717926
5.081504	519.964115	5.722931
5.424884	521.520841	5.727936
5.569595	528.759497	5.732941
4.936985	523.502337	5.737946
5.357780	533.103138	5.742950
5.391513	535.947427	5.747955
5.586378	545.653942	5.752960
5.373991	544.747643	5.757965
5.602531	537.875785	5.762970
5.391608	522.952500	5.767974
5.312598	522.162875	5.772979
5.403054	522.305294	5.777984
5.149749	552.461475	5.782989
4.976702	543.616995	5.787994
5.480039	543.290136	5.792998
5.418221	547.389866	5.798003
5.775160	544.349219	5.803008
5.427676	553.906017	5.808013
5.450275	552.889753	5.813018
5.519478	557.486977	5.818022
5.584692	553.138667	5.823027
5.692638	542.409047	5.828032
5.451528	544.517970	5.833037
5.755640	545.294877	5.838042
5.637042	546.760722	5.843046
5.453481	547.467566	5.848051
5.818781	542.922963	5.853056
5.448735	538.823579	5.858061
5.583465	535.034232	5.863066
5.908848	537.707693	5.868070
5.780445	551.796189	5.873075
5.495817	542.979324	5.878080
5.352840	547.576781	5.883085
5.325053	548.272879	5.888090
5.625460	550.198295	5.893094
5.746921	552.478856	5.898099
5.786211	551.688327	5.903104
5.517815	557.187438	5.908109
5.552328	544.817415	5.913114
5.742369	554.496516	5.918118
5.720885	555.530565	5.923123
5.936197	562.002928	5.928128
5.697436	569.163891	5.933133
6.155314	574.569135	5.938138
5.665249	563.506789	5.943142
5.555467	564.055031	5.948147
5.732721	570.783689	5.953152
5.747256	584.218065	5.958157
5.720211	580.919828	5.963162
6.007007	580.822717	5.968166
5.792577	587.796655	5.973171
6.113540	581.859494	5.978176
5.812128	587.308921	5.983181
5.714615	583.937384	5.988186
6.163597	577.624685	5.993190
5.733799	591.340467	5.998195
5.613433	590.064674	6.003200
5.684444	583.629743	6.008205
5.625180	586.729941	6.013210
6.010141	575.358916	6.018214
5.884623	587.629175	6.023219
6.012985	582.962507	6.028224
5.816517	585.364179	6.033229
6.288806	599.552647	6.038234
6.113718	586.144900	6.043238
6.179473	586.079186	6.048243
6.027845	573.485063	6.053248
5.916097	580.518589	6.058253
6.152403	568.259045	6.063258
6.132989	573.490693	6.068262
6.156088	582.242677	6.073267
6.344508	584.173974	6.078272
6.056360	576.861926	6.083277
6.159426	580.861804	6.088282
6.151540	575.643161	6.093286
6.056673	574.960536	6.098291
6.375497	571.946309	6.103296
6.354904	587.893615	6.108301
6.407716	579.055103	6.113306
5.938116	573.980440	6.118310
6.140115	582.445655	6.123315
6.379653	562.419831	6.128320
5.615042	557.507876	6.133325
5.826001	552.715885	6.138330
5.706355	554.812334	6.143334
6.076500	574.501713	6.148339
6.494043	573.406566	6.153344
6.260781	556.925858	6.158349
6.110446	553.854198	6.163354
5.855635	556.310496	6.168358
5.601837	565.204715	6.173363
6.031116	559.402980	6.178368
6.101314	566.320599	6.183373
5.905816	551.624217	6.188378
6.150179	562.240782	6.193382
6.123965	564.380198	6.198387
6.220291	554.354350	6.203392
5.533933	556.855324	6.208397
6.072966	549.967077	6.213402
6.212920	552.613862	6.218406
5.980853	557.605685	6.223411
6.208461	554.059570	6.228416
6.090556	549.053277	6.233421
6.152616	550.440728	6.238426
6.184074	549.396757	6.243430
5.698793	554.689106	6.248435
5.888133	555.225309	6.253440
6.088745	552.716121	6.258445
5.909670	548.857178	6.263450
6.280258	550.016157	6.268454
5.773207	556.398141	6.273459
6.151148	552.794133	6.278464
5.904735	545.714648	6.283469
5.927128	547.563175	6.288474
5.982066	549.853249	6.293478
5.918411	551.951594	6.298483
5.900527	540.832940	6.303488
5.532406	551.039954	6.308493
6.121426	566.006263	6.313498
6.072067	578.019157	6.318502
6.118473	585.583086	6.323507
6.061990	568.841796	6.328512
5.988276	565.450051	6.333517
6.112603	562.750723	6.338522
5.787574	551.359513	6.343526
5.603087	565.588901	6.348531
5.971097	575.117748	6.353536
6.199958	584.345600	6.358541
6.077640	579.328286	6.363546
6.216173	587.316912	6.368550
5.928977	587.492536	6.373555
6.071521	577.285988	6.378560
5.960439	568.957698	6.383565
5.906125	562.006289	6.388570
6.044594	573.601496	6.393574
6.003685	579.188615	6.398579
6.095026	584.369408	6.403584
6.256306	574.160061	6.408589
6.089696	565.130210	6.413594
5.912616	553.465336	6.418598
5.502885	569.308223	6.423603
6.223346	555.115372	6.428608
6.165608	571.848700	6.433613
5.556070	561.291895	6.438618
6.107633	573.371229	6.443622
5.706385	574.128648	6.448627
5.936885	579.914999	6.453632
5.945623	584.591679	6.458637
6.242066	583.275718	6.463642
6.143584	589.025770	6.468646
5.884588	584.109179	6.473651
6.119027	578.504789	6.478656
5.902872	581.713786	6.483661
6.251010	592.009845	6.488666
6.129701	581.636752	6.493670
6.119426	586.417009	6.498675
5.879181	569.673725	6.503680
5.795887	573.143916	6.508685
5.814477	590.001982	6.513690
6.213391	583.963244	6.518694
6.044049	579.071994	6.523699
6.211310	582.763314	6.528704
5.873881	574.212262	6.533709
6.023733	580.041143	6.538714
5.891015	591.101457	6.543718
6.066811	587.600400	6.548723
6.052321	582.182963	6.553728
5.748235	583.711034	6.558733
6.014490	582.525950	6.563738
6.446033	592.749229	6.568742
6.306269	574.616986	6.573747
6.323321	565.421523	6.578752
6.126114	556.823433	6.583757
5.980661	569.636834	6.588762
5.949099	553.089747	6.593766
5.611718	563.604241	6.598771
6.012892	555.414178	6.603776
5.847010	550.703108	6.608781
5.698169	547.600520	6.613786
6.141879	555.654031	6.618790
5.893250	571.387523	6.623795
6.394876	572.063026	6.628800
6.203135	567.939990	6.633805
6.174061	559.742688	6.638810
6.252481	557.709398	6.643814
5.887564	557.320217	6.648819
6.300825	549.636253	6.653824
5.925556	550.898064	6.658829
5.963085	551.499804	6.663834
6.150761	553.600420	6.668838
5.672135	552.635117	6.673843
5.967704	549.134304	6.678848
5.733963	553.153625	6.683853
5.726721	557.165806	6.688858
6.140533	558.214149	6.693862
5.754726	561.729987	6.698867
5.779243	561.954436	6.703872
6.219965	559.863247	6.708877
5.965836	567.664974	6.713882
6.238120	573.611546	6.718886
6.118790	563.747219	6.723891
5.967781	561.057973	6.728896
5.872367	558.971423	6.733901
5.904995	563.172855	6.738906
6.160420	557.984897	6.743910
6.166018	565.505539	6.748915
6.032693	559.304565	6.753920
6.390624	550.617700	6.758925
6.088090	552.664261	6.763930
6.289863	547.439197	6.768934
5.900437	549.421091	6.773939
5.995847	560.874922	6.778944
6.080089	552.572276	6.783949
6.068160	553.480633	6.788954
6.154697	548.398133	6.793958
5.848534	549.564269	6.798963
6.010804	549.974617	6.803968
5.896742	557.324223	6.808973
6.003324	549.299657	6.813978
5.869315	545.093389	6.818982
5.750495	558.377619	6.823987
5.861602	564.544885	6.828992
6.091222	554.762205	6.833997
5.935860	555.798349	6.839002
6.020682	550.445314	6.844006
5.972202	559.530641	6.849011
6.013438	558.662935	6.854016
5.773790	558.555542	6.859021
5.707786	563.575568	6.864026
6.141515	557.729095	6.869030
5.840430	563.958754	6.874035
6.114921	562.414079	6.879040
6.128616	571.380615	6.884045
5.644971	565.264069	6.889050
5.911734	565.541127	6.894054
6.254170	595.640382	6.899059
6.219807	596.412253	6.904064
5.905410	573.695173	6.909069
5.822307	583.254176	6.914074
5.652244	578.819146	6.919078
6.023698	583.767381	6.924083
6.065242	598.379439	6.929088
6.200094	588.663799	6.934093
6.120690	596.764117	6.939098
6.208857	588.893719	6.944102
5.868773	578.625349	6.949107
6.150456	582.768068	6.954112
6.212718	574.919323	6.959117
5.945721	568.729089	6.964122
6.359964	577.098848	6.969126
5.819798	577.203213	6.974131
6.097463	569.892971	6.979136
6.047537	571.920777	6.984141
5.870263	568.842221	6.989146
5.750107	572.668742	6.994150
6.042220	574.722308	6.999155
6.054413	563.321140	7.004160
5.897284	571.499896	7.009165
6.273059	576.919202	7.014170
6.086278	569.426928	7.019174
5.942123	566.240590	7.024179
5.911566	559.971626	7.029184
6.092312	564.598763	7.034189
5.797282	576.325099	7.039194
5.936038	561.969785	7.044198
5.976418	567.820798	7.049203
5.949279	571.999946	7.054208
5.705779	569.437270	7.059213
5.920424	588.402555	7.064218
6.109064	597.016889	7.069222
6.254269	604.146087	7.074227
5.900613	581.909836	7.079232
6.243054	583.617277	7.084237
5.982273	575.982236	7.089242
5.915003	566.654592	7.094246
6.015973	559.158281	7.099251
6.000161	560.527721	7.104256
5.696248	569.448772	7.109261
6.140482	584.043206	7.114266
6.085149	584.377043	7.119270
6.304239	574.601912	7.124275
6.232536	570.396587	7.129280
6.113760	562.563459	7.134285
5.970301	563.744836	7.139290
6.166758	559.238687	7.144294
6.278691	564.155808	7.149299
5.880568	561.454023	7.154304
6.259471	566.599030	7.159309
5.760008	563.078745	7.164314
6.134723	561.491462	7.169318
6.043794	564.409929	7.174323
5.920059	566.005276	7.179328
5.845123	567.653826	7.184333
5.848297	563.220856	7.189338
6.074421	557.458415	7.194342
6.079790	568.515230	7.199347
6.158653	567.406004	7.204352
6.150346	567.291458	7.209357
6.002846	564.388528	7.214362
6.081878	550.905374	7.219366
5.611129	563.519367	7.224371
5.899315	571.842077	7.229376
5.824684	557.721025	7.234381
5.993725	571.790872	7.239386
6.111881	559.306481	7.244390
6.034051	569.487143	7.249395
5.730213	561.070544	7.254400
5.857595	566.819570	7.259405
5.396792	563.090152	7.264410
6.086682	575.122062	7.269414
6.159952	585.995213	7.274419
6.222899	589.227643	7.279424
6.121243	580.333164	7.284429
5.867501	575.428040	7.289434
5.694620	566.332038	7.294438
5.574068	576.180475	7.299443
5.832236	584.695999	7.304448
6.110662	595.687881	7.309453
5.882773	594.667624	7.314458
6.123696	588.490133	7.319462
6.143356	590.652162	7.324467
6.175675	605.526803	7.329472
6.299322	594.289713	7.334477
6.376976	595.012391	7.339482
6.030481	572.451269	7.344486
5.893437	569.333902	7.349491
5.760951	569.837060	7.354496
5.889241	577.717468	7.359501
5.920657	586.943221	7.364506
6.271908	580.722836	7.369510
6.071855	601.952325	7.374515
6.270749	589.608279	7.379520
6.288682	577.801057	7.384525
5.900655	566.181096	7.389530
6.296761	559.931504	7.394534
6.064528	566.450301	7.399539
5.761393	564.624203	7.404544
6.041183	555.050775	7.409549
6.007129	560.777344	7.414554
6.175147	555.348107	7.419558
6.452137	570.110952	7.424563
6.101356	565.205687	7.429568
6.091014	558.286773	7.434573
6.047540	563.614640	7.439578
6.361399	555.684075	7.444582
6.171506	567.259644	7.449587
6.185432	568.859965	7.454592
6.137632	564.796016	7.459597
6.067958	573.781658	7.464602
6.418966	559.637919	7.469606
5.692140	553.606157	7.474611
5.979672	560.687248	7.479616
5.876964	560.404205	7.484621
6.115885	575.119182	7.489626
5.997782	562.439515	7.494630
5.886130	562.630921	7.499635
5.983839	559.437568	7.504640
6.140851	564.943139	7.509645
5.883526	566.744068	7.514650
6.184424	557.720331	7.519654
5.972632	562.609159	7.524659
6.060090	557.726091	7.529664
6.043003	569.001201	7.534669
5.875809	564.363746	7.539674
6.297544	556.597675	7.544678
5.891847	562.820055	7.549683
6.129036	555.282292	7.554688
5.878215	559.029278	7.559693
5.341756	562.130683	7.564698
6.315262	559.374691	7.569702
5.728204	562.276287	7.574707
5.786269	569.715648	7.579712
5.943677	568.560885	7.584717
6.093648	576.442938	7.589722
6.173614	560.586278	7.594726
6.122772	569.423184	7.599731
5.884856	561.909175	7.604736
6.297702	567.929894	7.609741
6.213124	576.533525	7.614746
6.194481	570.710895	7.619750
6.392829	563.340164	7.624755
5.885695	548.160553	7.629760
6.012803	535.507081	7.634765
5.765000	538.826074	7.639770
5.845437	551.278531	7.644774
5.872191	566.612620	7.649779
6.094108	551.596272	7.654784
6.196754	561.655647	7.659789
5.690485	571.954960	7.664794
6.335900	562.712192	7.669798
5.967469	562.862171	7.674803
5.969424	558.042167	7.679808
6.120008	560.848603	7.684813
5.778198	564.040574	7.689818
5.969644	555.326266	7.694822
5.825316	567.391546	7.699827
5.951025	570.253101	7.704832
5.724051	556.046530	7.709837
5.970776	568.824720	7.714842
6.100253	563.425824	7.719846
5.970532	575.047000	7.724851
6.420209	570.551785	7.729856
6.207514	567.241807	7.734861
5.770625	572.884495	7.739866
6.271997	568.840193	7.744870
6.198675	566.449082	7.749875
6.184396	555.928286	7.754880
6.254291	538.109213	7.759885
5.765220	542.124947	7.764890
5.994121	530.880080	7.769894
5.841938	530.289702	7.774899
6.085742	535.692029	7.779904
6.162650	531.803812	7.784909
5.890591	538.068325	7.789914
5.897456	540.798960	7.794918
6.111095	539.601362	7.799923
6.060437	536.678883	7.804928
5.989369	532.468235	7.809933
5.957248	544.195991	7.814938
6.286355	526.876126	7.819942
6.454115	531.086395	7.824947
6.471251	537.392305	7.829952
6.331379	537.283715	7.834957
6.343382	539.565295	7.839962
6.159480	531.856895	7.844966
6.032973	540.203622	7.849971
6.153752	531.718153	7.854976
6.072693	540.730618	7.859981
5.530839	544.351560	7.864986
5.951545	527.617884	7.869990
5.877965	542.204221	7.874995
5.937839	539.247887	7.880000
5.758737	533.517000	7.885005
5.653376	540.124134	7.890010
5.862370	531.610769	7.895014
5.601841	529.655593	7.900019
5.777082	536.563832	7.905024
5.787991	542.734821	7.910029
5.918519	540.208211	7.915034
6.337762	543.871989	7.920038
6.086353	540.855414	7.925043
5.980931	538.303371	7.930048
6.273469	537.481648	7.935053
5.692712	539.767160	7.940058
5.964882	543.652856	7.945062
6.008638	541.836130	7.950067
5.571129	543.316987	7.955072
6.151453	547.538898	7.960077
6.137778	552.368247	7.965082
6.223298	541.810744	7.970086
6.196032	546.182982	7.975091
6.121801	534.644774	7.980096
6.307477	534.034772	7.985101
5.887195	539.073575	7.990106
5.837816	535.489476	7.995110
5.910704	533.865353	8.000115
6.099708	532.179872	8.005133
6.133055	535.154527	8.010150
6.038767	547.960977	8.015168
6.115588	534.691764	8.020186
5.934322	535.810894	8.025203
5.901554	542.886277	8.030221
5.876686	546.264381	8.035238
5.794761	540.338069	8.040256
5.722102	532.143225	8.045274
5.658716	540.438699	8.050291
5.971165	553.492251	8.055309
6.039029	565.246614	8.060326
6.093179	566.286694	8.065344
6.221997	563.945854	8.070362
6.038500	573.852244	8.075379
5.796078	573.149434	8.080397
6.368595	569.769698	8.085414
6.124500	570.010399	8.090432
6.103546	560.777752	8.095450
6.237699	565.304269	8.100467
5.841069	558.387036	8.105485
5.866292	556.811408	8.110502
6.009427	568.406315	8.115520
5.962101	568.272730	8.120538
6.315201	570.635206	8.125555
5.918468	567.054192	8.130573
6.073203	566.799338	8.135590
6.205425	573.934660	8.140608
6.439916	569.270377	8.145626
6.319210	573.747887	8.150643
6.037090	570.205303	8.155661
6.093928	564.309192	8.160678
6.197615	565.688857	8.165696
6.094612	565.294935	8.170714
5.832042	557.581379	8.175731
5.710451	566.900277	8.180749
6.164113	573.091696	8.185766
5.910457	569.049223	8.190784
6.286158	567.707258	8.195802
5.801157	559.484198	8.200819
5.771144	560.159810	8.205837
6.185953	582.908583	8.210854
6.082580	598.981833	8.215872
6.297911	600.125374	8.220890
5.969917	595.464878	8.225907
6.152282	586.113298	8.230925
6.452551	589.947236	8.235942
6.199478	598.064971	8.240960
6.270656	596.845066	8.245978
6.427565	602.205084	8.250995
6.172447	603.876976	8.256013
6.190059	592.200580	8.261030
6.175045	598.463063	8.266048
6.393233	599.412564	8.271066
6.047195	606.822568	8.276083
6.157091	605.792095	8.281101
6.249440	594.446592	8.286118
6.097164	607.311287	8.291136
6.097977	605.182308	8.296154
6.040473	613.153482	8.301171
6.072843	605.201432	8.306189
6.068981	603.474433	8.311206
6.003418	609.659463	8.316224
6.299892	613.197629	8.321242
6.325794	616.954592	8.326259
6.573403	626.135265	8.331277
6.528999	608.849830	8.336294
6.309869	604.031898	8.341312
6.172701	609.274797	8.346330
6.642156	605.219001	8.351347
6.171973	608.580763	8.356365
6.281198	594.570744	8.361382
6.325322	610.483632	8.366400
6.157367	598.750117	8.371418
6.358531	606.724892	8.376435
6.344306	634.378912	8.381453
6.398868	633.839189	8.386470
6.604889	630.320926	8.391488
6.246659	632.662008	8.396506
6.851047	625.533368	8.401523
6.401969	616.004179	8.406541
6.424099	601.618557	8.411558
6.501362	607.403377	8.416576
6.101722	594.865389	8.421594
6.675979	606.348536	8.426611
6.069423	613.695511	8.431629
6.514051	615.442976	8.436646
6.461954	625.400998	8.441664
6.312768	628.175365	8.446682
6.643725	622.732663	8.451699
6.086993	622.347196	8.456717
6.159709	623.569415	8.461734
6.077583	638.308329	8.466752
6.177215	627.061679	8.471770
6.381241	625.928067	8.476787
6.164893	624.211184	8.481805
6.730378	627.034547	8.486822
6.425818	626.315924	8.491840
6.327712	623.591194	8.496858
6.444345	627.305907	8.501875
6.298318	629.429769	8.506893
6.434493	627.710527	8.511910
6.823301	639.596031	8.516928
6.856356	639.831378	8.521946
6.874219	628.411167	8.526963
6.895886	633.812145	8.531981
6.810286	626.137702	8.536998
6.508758	627.185489	8.542016
6.707918	623.563458	8.547034
6.785716	624.403999	8.552051
6.720299	636.411110	8.557069
6.815486	627.764537	8.562087
6.795354	625.238989	8.567104
6.834513	633.405284	8.572122
6.825808	622.472649	8.577139
6.090940	630.494656	8.582157
6.471403	625.118365	8.587175
6.910800	624.613554	8.592192
6.549115	639.823591	8.597210
6.971145	626.185596	8.602227
6.544550	628.084512	8.607245
6.908865	625.861510	8.612263
6.747103	620.967766	8.617280
6.562348	623.872004	8.622298
6.716950	635.591225	8.627315
6.686144	619.970361	8.632333
6.603350	633.176091	8.637351
6.789715	631.125777	8.642368
6.409388	618.273806	8.647386
6.600373	621.948973	8.652403
6.467500	627.682222	8.657421
6.620905	624.035869	8.662439
6.720663	620.551898	8.667456
6.643121	626.117075	8.672474
6.531992	617.039429	8.677491
6.419430	632.400974	8.682509
6.210503	626.438441	8.687527
6.451385	628.315426	8.692544
6.480619	620.979230	8.697562
6.426444	623.270459	8.702579
6.483121	646.885353	8.707597
6.746590	646.671280	8.712615
6.743473	654.948196	8.717632
6.885894	654.265826	8.722650
7.090823	655.902146	8.727667
6.909262	653.647912	8.732685
6.927976	651.753820	8.737703
7.076490	638.020978	8.742720
6.667415	637.231650	8.747738
6.768282	618.069672	8.752755
6.739383	613.558332	8.757773
6.935333	619.254264	8.762791
6.758852	611.213223	8.767808
6.886667	619.298238	8.772826
7.080473	617.427864	8.777843
6.883381	625.980870	8.782861
6.703707	618.322075	8.787879
6.517198	618.475814	8.792896
6.324348	631.101116	8.797914
7.108095	635.027973	8.802931
6.921197	644.677338	8.807949
6.752366	646.994013	8.812967
7.024489	637.167907	8.817984
6.807540	650.675595	8.823002
7.068864	645.757588	8.828019
6.911315	659.294142	8.833037
6.532151	661.540379	8.838055
7.107117	645.865143	8.843072
6.593160	648.108755	8.848090
7.177026	645.990094	8.853107
7.005305	658.412258	8.858125
7.015997	649.266340	8.863143
7.297891	642.767851	8.868160
7.000943	661.690078	8.873178
7.324091	648.675875	8.878195
7.065944	637.437957	8.883213
6.787086	632.132533	8.888231
7.307775	615.984296	8.893248
6.759678	620.327562	8.898266
6.746078	620.948505	8.903283
6.565410	630.384960	8.908301
7.029620	647.637764	8.913319
7.077397	647.200324	8.918336
7.137450	654.567354	8.923354
7.380332	648.325856	8.928371
6.987612	649.159030	8.933389
6.987592	662.605983	8.938407
7.050991	653.132610	8.943424
6.967842	656.058934	8.948442
7.061786	652.794776	8.953459
7.040888	658.747483	8.958477
7.091387	655.775197	8.963495
6.994233	657.970599	8.968512
6.856775	657.608250	8.973530
7.001615	655.487938	8.978547
6.913010	654.273768	8.983565
7.168135	668.611174	8.988583
7.010380	654.145898	8.993600
7.266390	661.417174	8.998618
7.143452	654.006126	9.003635
6.699145	657.926416	9.008653
6.893941	658.053948	9.013671
7.064208	653.672843	9.018688
6.948201	654.212106	9.023706
6.937975	645.902079	9.028723
7.028330	646.804118	9.033741
6.623456	650.148601	9.038759
7.324451	648.709476	9.043776
7.045934	648.612324	9.048794
6.901540	651.442980	9.053811
7.365383	661.300709	9.058829
6.969939	665.307202	9.063847
6.993564	666.787788	9.068864
7.217280	684.178192	9.073882
7.156131	691.308620	9.078899
7.202146	695.131262	9.083917
7.247766	688.100737	9.088935
7.320982	688.883880	9.093952
7.248977	689.240508	9.098970
7.416406	695.522381	9.103987
7.470445	679.871395	9.109005
7.335420	672.640552	9.114023
7.591010	660.824106	9.119040
7.107665	670.128254	9.124058
7.180182	664.972689	9.129075
6.854009	658.824142	9.134093
7.120653	664.933729	9.139111
7.530680	672.664906	9.144128
7.547521	679.653329	9.149146
7.119404	667.949370	9.154163
6.845259	667.909162	9.159181
7.178915	673.966347	9.164199
7.274980	682.758783	9.169216
7.178203	699.015267	9.174234
7.310007	692.151569	9.179251
7.615798	691.438460	9.184269
7.394676	694.725034	9.189287
7.335050	690.960155	9.194304
6.981479	695.465160	9.199322
7.196512	696.425620	9.204339
7.558084	689.772631	9.209357
7.121769	700.032636	9.214375
7.500977	693.697837	9.219392
7.298756	710.020961	9.224410
7.598242	698.819566	9.229427
7.536537	691.204910	9.234445
7.372989	698.242538	9.239463
7.569846	700.338385	9.244480
7.729343	701.143386	9.249498
7.405413	703.364755	9.254515
7.534892	695.569416	9.259533
7.491505	705.055659	9.264551
7.736670	694.400848	9.269568
7.571357	691.069504	9.274586
7.215788	675.695524	9.279603
7.509185	681.991411	9.284621
7.233495	690.653487	9.289639
7.678718	691.822716	9.294656
7.434868	694.870370	9.299674
7.716205	701.306226	9.304691
7.744266	689.385060	9.309709
7.418216	682.094162	9.314727
7.914681	666.386118	9.319744
7.439854	671.371900	9.324762
7.749794	664.055918	9.329779
7.734301	659.909607	9.334797
7.266238	661.963287	9.339815
7.516982	665.124641	9.344832
7.408387	663.977345	9.349850
7.168197	659.252722	9.354867
7.305641	670.565428	9.359885
7.424592	694.945364	9.364903
8.145620	694.336146	9.369920
7.659647	685.986724	9.374938
7.527730	675.000411	9.379955
7.354298	662.019545	9.384973
7.597463	673.482765	9.389991
7.794630	684.972489	9.395008
7.271089	682.327696	9.400026
7.415894	693.621981	9.405043
7.841818	696.992148	9.410061
7.433167	697.147464	9.415079
7.798247	693.770491	9.420096
7.509151	699.520333	9.425114
7.250352	692.452529	9.430131
7.647497	687.572782	9.435149
8.049515	694.397873	9.440167
7.830263	700.894310	9.445184
7.828912	689.637044	9.450202
7.602631	693.423201	9.455219
7.716037	694.075118	9.460237
7.392812	695.546697	9.465255
7.511534	697.368596	9.470272
7.646333	696.464983	9.475290
7.307268	702.849550	9.480307
7.588834	694.304204	9.485325
7.226009	692.470402	9.490343
7.677942	704.469224	9.495360
7.836221	691.849194	9.500378
7.308746	696.437652	9.505395
7.589225	687.312275	9.510413
7.333542	705.425415	9.515431
7.580409	719.550984	9.520448
7.681780	718.078484	9.525466
7.834688	725.366336	9.530483
8.118664	719.215542	9.535501
7.949957	723.887708	9.540519
8.095947	734.023857	9.545536
7.837615	724.655172	9.550554
7.767512	712.586262	9.555571
8.144651	698.573009	9.560589
7.957845	697.583983	9.565607
7.849720	703.676298	9.570624
7.684722	696.047907	9.575642
7.543737	701.984065	9.580659
8.050940	704.364888	9.585677
7.855402	715.332132	9.590695
7.857560	718.163676	9.595712
7.718135	711.872455	9.600730
7.807023	722.951139	9.605747
7.904925	711.782653	9.610765
7.583899	724.873920	9.615783
7.696293	727.694433	9.620800
8.068301	722.410140	9.625818
7.610293	734.996780	9.630835
7.941436	732.774127	9.635853
7.655797	738.058433	9.640871
7.818234	735.363351	9.645888
8.024499	729.568446	9.650906
7.723818	730.920870	9.655923
7.957883	728.813259	9.660941
7.922585	725.089226	9.665959
7.749797	728.310939	9.670976
7.808840	733.072813	9.675994
7.935314	738.102237	9.681011
8.219546	732.199384	9.686029
7.397837	738.813796	9.691047
7.864903	750.152982	9.696064
8.181018	760.203564	9.701082
7.993964	767.860554	9.706099
8.001592	754.769586	9.711117
8.227905	761.863269	9.716135
8.185281	758.422674	9.721152
8.143635	743.957020	9.726170
7.786255	745.959257	9.731187
8.290990	740.627536	9.736205
8.151423	743.777435	9.741223
7.984010	746.489689	9.746240
8.224813	734.492492	9.751258
8.240057	731.811894	9.756275
8.304809	724.105668	9.761293
7.967438	735.875758	9.766311
8.123528	724.981555	9.771328
8.395403	731.757709	9.776346
8.106184	729.740311	9.781363
8.290068	722.861498	9.786381
7.900522	727.790791	9.791399
8.035879	733.677063	9.796416
8.208312	719.335281	9.801434
7.928475	725.371053	9.806451
8.080164	713.193357	9.811469
7.724865	731.448362	9.816487
8.033430	743.393557	9.821504
8.333552	747.455866	9.826522
8.124975	766.091124	9.831539
8.226479	756.781047	9.836557
8.187082	760.221825	9.841575
8.180323	767.019830	9.846592
8.631832	766.303206	9.851610
8.306174	764.777767	9.856627
8.684790	753.618660	9.861645
8.345402	747.128422	9.866663
8.072533	737.198251	9.871680
8.235444	739.511685	9.876698
8.473933	755.517386	9.881715
8.525691	745.230270	9.886733
8.205472	733.555273	9.891751
7.981095	741.774228	9.896768
8.246846	740.967653	9.901786
8.227876	760.541289	9.906803
8.340283	762.706208	9.911821
8.534904	757.377115	9.916839
8.388530	757.478068	9.921856
8.643695	745.035455	9.926874
8.130087	742.289912	9.931891
8.330213	741.660099	9.936909
8.222598	753.342046	9.941927
8.609408	760.944549	9.946944
8.406003	747.883736	9.951962
8.273862	755.369862	9.956979
8.470365	756.413001	9.961997
8.259462	757.576408	9.967015
8.638446	759.855909	9.972032
8.587530	751.164426	9.977050
8.175813	746.419705	9.982067
8.461305	746.560887	9.987085
8.302638	759.243823	9.992103
8.541208	764.311218	9.997120
8.523600	756.369809	10.002138
8.249624	766.568097	10.007155
8.651757	761.451323	10.012173
8.490142	760.467971	10.017191
8.523121	767.500904	10.022208
8.684626	763.990361	10.027226
8.497914	768.265780	10.032243
8.322585	776.926967	10.037261
8.376802	765.778159	10.042279
8.261189	773.672320	10.047296
8.290607	761.922794	10.052314
8.290200	775.002353	10.057331
8.097309	768.916368	10.062349
8.436504	764.357932	10.067367
8.123747	758.556675	10.072384
8.183815	761.765305	10.077402
7.989334	772.086854	10.082419
8.358021	787.741601	10.087437
8.305236	790.470347	10.092455
8.602917	800.139617	10.097472
8.541964	798.702299	10.102490
8.629027	795.684679	10.107507
8.645056	800.086222	10.112525
8.903602	793.338323	10.117543
8.463707	803.289690	10.122560
8.776099	798.624472	10.127578
8.568686	801.179199	10.132595
8.448927	802.311999	10.137613
8.668168	796.580465	10.142631
8.189410	803.065015	10.147648
8.727165	797.969313	10.152666
8.247914	805.517941	10.157683
8.488080	797.669325	10.162701
8.661447	796.864827	10.167719
8.390900	804.094171	10.172736
8.822211	818.712197	10.177754
8.880138	813.075806	10.182771
8.944040	820.655925	10.187789
8.796048	800.303454	10.192807
8.761497	802.128552	10.197824
9.025121	808.364461	10.202842
8.745047	799.487432	10.207859
8.567549	787.256614	10.212877
8.782738	798.801408	10.217895
8.630444	801.509795	10.222912
8.687144	799.959153	10.227930
8.477830	812.393852	10.232947
8.643565	826.653280	10.237965
8.979832	827.487728	10.242983
8.989483	831.054843	10.248000
8.935924	814.594766	10.253018
9.064528	832.942338	10.258035
8.906319	821.706172	10.263053
8.977698	829.729671	10.268071
8.851009	824.499904	10.273088
8.920620	818.021759	10.278106
9.001336	807.762291	10.283123
8.889681	813.793727	10.288141
8.776127	789.617315	10.293159
8.591179	804.580432	10.298176
8.688970	814.577379	10.303194
8.826767	826.628602	10.308211
8.918895	834.389465	10.313229
9.284151	826.932496	10.318247
8.943808	830.794810	10.323264
8.878265	837.584060	10.328282
8.916716	829.962232	10.333299
8.849136	841.109961	10.338317
8.946937	836.457559	10.343335
8.635316	827.979165	10.348352
8.987785	829.397454	10.353370
8.898453	835.963506	10.358387
8.617686	834.181864	10.363405
9.015737	820.935588	10.368423
8.983591	828.023398	10.373440
8.911573	830.306584	10.378458
8.999166	832.531904	10.383475
8.893734	840.906031	10.388493
9.090317	821.787521	10.393511
8.897111	832.083903	10.398528
8.896484	828.318492	10.403546
9.344516	841.780620	10.408563
8.833037	840.577368	10.413581
9.264051	834.968279	10.418599
8.957625	833.569554	10.423616
9.281322	837.225695	10.428634
9.231125	835.396897	10.433651
9.100660	840.977983	10.438669
9.254474	831.308683	10.443687
9.174109	831.604403	10.448704
8.854078	833.322572	10.453722
9.301022	846.842946	10.458739
9.065906	844.289317	10.463757
9.051313	839.414975	10.468775
9.069148	848.078724	10.473792
9.153112	854.848393	10.478810
9.297847	857.024319	10.483827
9.258603	865.004513	10.488845
9.261463	858.819423	10.493863
9.055427	871.375261	10.498880
9.156901	866.884618	10.503898
9.378147	853.345340	10.508915
9.078056	863.661571	10.513933
9.359003	862.739308	10.518951
8.899038	863.015095	10.523968
9.583868	867.952293	10.528986
9.545849	864.849638	10.534003
9.332928	862.706049	10.539021
9.290782	851.223161	10.544039
9.274716	864.805893	10.549056
9.491243	865.416666	10.554074
9.677931	863.517818	10.559091
9.373995	867.571140	10.564109
9.607105	853.234755	10.569127
9.328739	851.630637	10.574144
9.152234	843.621756	10.579162
9.898610	842.792632	10.584179
9.483178	833.172919	10.589197
9.576647	829.358105	10.594215
9.478358	833.906875	10.599232
9.303858	833.993779	10.604250
8.947784	839.422020	10.609267
8.737316	843.742127	10.614285
9.234284	850.501409	10.619303
9.606115	866.169494	10.624320
9.386122	869.968236	10.629338
9.602498	863.489634	10.634355
9.116155	867.783891	10.639373
9.609953	863.122726	10.644391
9.493101	873.846801	10.649408
9.370544	873.492318	10.654426
9.694071	871.997952	10.659443
9.428407	877.234523	10.664461
9.367770	862.910653	10.669479
9.306265	863.580952	10.674496
9.409446	867.957485	10.679514
9.697600	873.613279	10.684531
9.221826	881.934473	10.689549
9.442802	865.623235	10.694567
9.816950	867.917920	10.699584
9.623852	858.326204	10.704602
9.352418	864.987508	10.709619
9.305572	879.396072	10.714637
9.694953	865.291094	10.719655
9.576665	852.105317	10.724672
9.609410	874.126056	10.729690
9.593432	863.078330	10.734707
9.428957	876.925322	10.739725
9.692575	865.357058	10.744743
9.334091	882.071285	10.749760
9.366099	894.392757	10.754778
9.598432	902.548923	10.759795
9.479478	909.140961	10.764813
9.617835	896.167420	10.769831
9.878150	905.828957	10.774848
9.905035	905.552713	10.779866
10.008338	898.926864	10.784883
9.975024	898.559404	10.789901
10.192533	887.502008	10.794919
9.955853	876.816872	10.799936
9.636918	876.871747	10.804954
9.939910	863.229006	10.809971
9.608459	860.613943	10.814989
9.497578	860.382313	10.820007
9.775493	861.828080	10.825024
9.729599	868.431252	10.830042
9.967786	870.582487	10.835059
9.533696	864.100567	10.840077
9.862276	873.403615	10.845095
10.200117	874.083500	10.850112
9.552160	877.331215	10.855130
10.021574	869.216172	10.860147
9.659769	876.962321	10.865165
9.699143	887.349419	10.870183
9.897910	892.600571	10.875200
9.724870	898.426667	10.880218
9.965722	888.268812	10.885235
9.849812	900.110287	10.890253
9.810867	896.502741	10.895271
10.317231	896.030156	10.900288
9.856010	902.657889	10.905306
9.815559	895.288006	10.910323
9.755807	898.392665	10.915341
9.931546	899.085955	10.920359
9.814759	906.211801	10.925376
9.656678	906.553628	10.930394
10.085546	893.383483	10.935411
9.782694	902.472835	10.940429
9.828286	898.029797	10.945447
9.931282	908.730556	10.950464
9.912985	905.014495	10.955482
10.186240	903.979740	10.960499
10.147932	909.903832	10.965517
10.037270	904.886315	10.970535
10.075237	901.816364	10.975552
9.907410	897.836085	10.980570
10.252142	906.209073	10.985587
10.243236	908.942989	10.990605
9.839326	900.316250	10.995623
9.803920	887.528492	11.000640
9.866497	906.979209	11.005658
10.110385	896.038099	11.010675
10.070831	900.670278	11.015693
10.048788	904.856722	11.020711
10.262766	904.877461	11.025728
9.904535	896.709833	11.030746
10.286921	903.067471	11.035763
10.039235	926.873128	11.040781
10.123728	934.432580	11.045799
10.131196	931.762285	11.050816
10.077007	932.799627	11.055834
10.210668	925.671387	11.060851
10.252404	941.386421	11.065869
10.094086	942.403181	11.070887
10.099652	935.935571	11.075904
9.975398	932.105931	11.080922
10.160861	930.791240	11.085939
9.973373	931.150523	11.090957
10.320462	942.632887	11.095975
10.223010	934.459934	11.100992
10.103170	931.578037	11.106010
10.456432	934.662674	11.111027
10.178470	934.988687	11.116045
10.270113	939.667100	11.121063
10.540715	932.790396	11.126080
10.256840	934.440800	11.131098
10.510744	935.365822	11.136115
10.676504	941.954518	11.141133
10.274907	939.682871	11.146151
10.480957	934.219172	11.151168
10.197732	936.792945	11.156186
10.323618	927.446851	11.161203
10.493986	936.915824	11.166221
9.863263	936.954911	11.171239
10.334744	925.709086	11.176256
10.199575	930.145493	11.181274
10.491435	929.870336	11.186291
10.339829	933.125200	11.191309
10.530005	941.849878	11.196327
10.407818	924.072101	11.201344
10.229461	944.952618	11.206362
10.710579	953.465274	11.211379
10.964717	948.946427	11.216397
10.324538	946.131422	11.221415
10.574721	923.745780	11.226432
10.370568	936.945549	11.231450
10.407143	931.849764	11.236467
10.543312	951.779244	11.241485
10.475157	955.208285	11.246503
10.945599	965.581869	11.251520
10.377609	952.326052	11.256538
10.474621	954.915327	11.261555
10.855550	966.664318	11.266573
10.434172	977.502952	11.271591
10.932330	962.424743	11.276608
10.428592	958.709964	11.281626
10.752414	959.955074	11.286643
10.590652	960.463429	11.291661
10.751263	966.264331	11.296679
10.576036	959.179640	11.301696
10.382986	964.783316	11.306714
10.827850	971.918330	11.311731
10.754780	967.841284	11.316749
10.413898	973.151134	11.321767
10.698433	965.524002	11.326784
10.826017	973.010614	11.331802
10.547055	964.353350	11.336819
10.562928	962.310697	11.341837
10.478436	968.540428	11.346855
10.835740	959.457798	11.351872
10.620475	968.815938	11.356890
10.834778	968.027104	11.361907
10.776418	969.020853	11.366925
10.552376	967.818508	11.371943
10.790511	956.051663	11.376960
10.620726	971.580064	11.381978
10.735365	970.365839	11.386995
10.669377	974.647346	11.392013
10.641602	970.339226	11.397031
10.967422	962.513177	11.402048
10.832529	967.804337	11.407066
10.835779	965.799394	11.412083
10.761484	975.031109	11.417101
10.993802	993.711875	11.422119
10.950507	988.741458	11.427136
11.244460	993.568907	11.432154
11.256112	979.469757	11.437171
10.716683	965.885834	11.442189
10.627137	959.096188	11.447207
11.106941	960.694597	11.452224
10.718670	972.906478	11.457242
10.838293	979.093823	11.462259
11.127672	990.851073	11.467277
11.038685	998.801373	11.472295
11.336873	992.122612	11.477312
11.134200	975.401813	11.482330
11.131489	966.522547	11.487347
11.347291	963.461969	11.492365
10.991023	965.360129	11.497383
11.330296	955.921875	11.502400
11.280825	967.306822	11.507418
11.415956	954.771098	11.512435
11.277179	954.173269	11.517453
11.559134	953.638766	11.522471
11.182795	967.494870	11.527488
11.114008	962.018123	11.532506
10.809771	960.796949	11.537523
11.371304	957.225965	11.542541
11.087111	956.174485	11.547559
11.656158	962.853609	11.552576
11.343755	964.778373	11.557594
11.091677	966.286342	11.562611
11.360395	955.902809	11.567629
10.928335	962.563538	11.572647
11.103253	959.413866	11.577664
11.214179	960.644953	11.582682
11.085943	966.664820	11.587699
11.322794	961.299155	11.592717
11.371657	964.626393	11.597735
11.526813	958.015568	11.602752
11.530002	971.373790	11.607770
10.898905	961.792193	11.612787
11.271475	966.166357	11.617805
10.859975	968.080336	11.622823
11.151230	967.768867	11.627840
10.801352	953.940475	11.632858
11.007927	960.725553	11.637875
11.199262	960.378439	11.642893
11.443233	970.311770	11.647911
11.437306	955.170041	11.652928
11.151897	953.733388	11.657946
11.182735	970.056064	11.662963
11.447592	971.248330	11.667981
11.396585	994.824573	11.672999
11.813108	992.729880	11.678016
11.388859	977.374033	11.683034
11.260550	982.232288	11.688051
11.317067	982.870098	11.693069
11.582903	999.440147	11.698087
11.630545	997.937038	11.703104
11.751855	992.343249	11.708122
11.282448	991.963613	11.713139
11.612578	979.834750	11.718157
11.343628	982.728956	11.723175
11.417045	991.163556	11.728192
11.274621	994.502925	11.733210
11.494084	997.985021	11.738227
11.575352	995.161793	11.743245
11.154024	1004.331207	11.748263
11.137079	993.158173	11.753280
11.683473	1001.393377	11.758298
11.189657	999.819729	11.763315
11.528073	985.954130	11.768333
11.400134	997.249523	11.773351
11.676897	986.767411	11.778368
11.657018	983.538919	11.783386
11.425554	997.715741	11.788403
11.576942	1000.313161	11.793421
11.545197	1013.154832	11.798439
11.460970	1018.984207	11.803456
11.696308	1027.044878	11.808474
11.840490	1022.746511	11.813491
12.075461	1025.002812	11.818509
11.779875	1015.442695	11.823527
11.733607	994.616534	11.828544
11.945641	993.449589	11.833562
11.725671	992.755547	11.838579
12.151672	982.027944	11.843597
11.807351	985.864186	11.848615
11.617473	988.250127	11.853632
11.680427	987.723865	11.858650
11.618529	986.443354	11.863667
11.945924	989.595849	11.868685
11.701071	996.699008	11.873703
12.079116	1002.958799	11.878720
11.926895	992.191526	11.883738
11.868982	996.007602	11.888755
11.650297	987.003014	11.893773
11.928417	997.051567	11.898791
12.019706	1012.449281	11.903808
12.030752	1008.812191	11.908826
12.082060	1012.252404	11.913843
11.891396	992.288169	11.918861
11.980806	996.215902	11.923879
11.803638	993.023241	11.928896
11.807449	996.530935	11.933914
11.751656	1017.496202	11.938931
12.164123	1023.457640	11.943949
11.888120	1023.993142	11.948967
11.962763	1028.026262	11.953984
12.276809	1013.546845	11.959002
11.923248	1026.609792	11.964019
12.112532	1017.919404	11.969037
11.975407	1024.363730	11.974055
12.102180	1026.718803	11.979072
12.089538	1023.659750	11.984090
11.827182	1025.149937	11.989107
12.143365	1022.384918	11.994125
11.718480	1030.260643	11.999143
11.847874	1025.779905	12.004160
11.999152	1020.910570	12.009178
12.291460	1019.642970	12.014195
12.620726	1017.735501	12.019213
12.392021	1030.273761	12.024231
12.370723	1029.832669	12.029248
12.326944	1019.551120	12.034266
12.028458	1022.655892	12.039283
12.309438	1023.598882	12.044301
12.293048	1014.449448	12.049319
11.847329	1022.076879	12.054336
12.393744	1027.420803	12.059354
11.889982	1028.507447	12.064371
12.212588	1025.236127	12.069389
12.243818	1036.192105	12.074407
12.302047	1022.147808	12.079424
12.485635	1013.498712	12.084442
12.078966	1025.585545	12.089459
12.441697	1023.874483	12.094477
12.176641	1025.001196	12.099495
12.295104	1032.311221	12.104512
12.682707	1021.546833	12.109530
12.492692	1019.048900	12.114547
12.653604	1021.852987	12.119565
12.370552	1020.659799	12.124583
12.337392	1031.509503	12.129600
12.163853	1023.772633	12.134618
12.506532	1022.219979	12.139635
12.357011	1021.358018	12.144653
12.537830	1022.632079	12.149671
12.407744	1028.271822	12.154688
12.227637	1022.532980	12.159706
12.478438	1024.028906	12.164723
12.438271	1019.725773	12.169741
12.449417	1028.027201	12.174759
12.536928	1032.606537	12.179776
12.426381	1023.593506	12.184794
12.482323	1024.786053	12.189811
12.326048	1028.431019	12.194829
12.531977	1024.743810	12.199847
12.445318	1043.482662	12.204864
12.570419	1033.418238	12.209882
12.920727	1040.668108	12.214899
12.715565	1028.989225	12.219917
12.619990	1028.150627	12.224935
12.678971	1029.827441	12.229952
12.670542	1022.613008	12.234970
12.436850	1022.346560	12.239987
12.474892	1023.618432	12.245005
12.284547	1034.346694	12.250023
12.431408	1043.804856	12.255040
12.752759	1037.663898	12.260058
12.747121	1041.490242	12.265075
12.802919	1030.175456	12.270093
12.814773	1033.268112	12.275111
12.473329	1046.740232	12.280128
12.840609	1026.365296	12.285146
12.792807	1049.856264	12.290163
12.482582	1044.340657	12.295181
12.913883	1050.401144	12.300199
12.385557	1046.393207	12.305216
12.784980	1043.806525	12.310234
12.554877	1050.828740	12.315251
12.390796	1058.665318	12.320269
12.408113	1056.343913	12.325287
13.020310	1065.731489	12.330304
13.169732	1069.719787	12.335322
12.966730	1076.082318	12.340339
13.310190	1065.395065	12.345357
12.803954	1050.820295	12.350375
12.738415	1054.101113	12.355392
12.914819	1053.156357	12.360410
13.148430	1067.019417	12.365427
13.184752	1066.444018	12.370445
12.584788	1051.356468	12.375463
12.626072	1066.804816	12.380480
12.863125	1066.226359	12.385498
13.056735	1075.797073	12.390515
12.950840	1061.008718	12.395533
13.183062	1068.704626	12.400551
12.708063	1085.697737	12.405568
12.776792	1074.514226	12.410586
12.856436	1070.971282	12.415603
13.006757	1076.778846	12.420621
12.856897	1076.747326	12.425639
12.416531	1078.489737	12.430656
12.985133	1082.033233	12.435674
12.949489	1096.328551	12.440691
13.071675	1101.497759	12.445709
13.483745	1102.976883	12.450727
13.229050	1105.900248	12.455744
13.497889	1101.382273	12.460762
13.600747	1093.844736	12.465779
13.063275	1082.375231	12.470797
12.954172	1074.354501	12.475815
13.265362	1083.612132	12.480832
13.503216	1077.684927	12.485850
13.596524	1073.481949	12.490867
13.498330	1068.975627	12.495885
13.454137	1066.320342	12.500903
13.328904	1074.149917	12.505920
13.482611	1063.374946	12.510938
13.467698	1062.802306	12.515955
13.093480	1064.848107	12.520973
13.517269	1057.478388	12.525991
13.136242	1074.613611	12.531008
13.381380	1065.285123	12.536026
13.537194	1055.135110	12.541043
13.514276	1065.419057	12.546061
13.794036	1066.307732	12.551079
13.252114	1081.302355	12.556096
13.531215	1059.965517	12.561114
13.511895	1070.205374	12.566131
13.444041	1076.038954	12.571149
13.567189	1066.708580	12.576167
12.995493	1077.189110	12.581184
13.582917	1065.261131	12.586202
13.485523	1057.952147	12.591219
13.257909	1071.380875	12.596237
13.631733	1075.135270	12.601255
13.276443	1078.088243	12.606272
13.085990	1061.299789	12.611290
13.229794	1083.662460	12.616307
13.443801	1094.144443	12.621325
13.937241	1094.181985	12.626343
13.732822	1106.188418	12.631360
13.694424	1102.387652	12.636378
13.718207	1091.858705	12.641395
13.922795	1107.704848	12.646413
14.036106	1090.372537	12.651431
13.739356	1082.571760	12.656448
13.641680	1071.872178	12.661466
13.495924	1058.304798	12.666483
13.517180	1069.420494	12.671501
13.773074	1083.881569	12.676519
13.482394	1103.788096	12.681536
13.424986	1102.702671	12.686554
13.858690	1104.488608	12.691571
13.754458	1104.359797	12.696589
13.805116	1106.240524	12.701607
14.068970	1105.459635	12.706624
13.849154	1099.437802	12.711642
14.236697	1099.586136	12.716659
14.094775	1097.389844	12.721677
14.352020	1086.899474	12.726695
13.785922	1077.758571	12.731712
14.042749	1068.219126	12.736730
13.892371	1060.062922	12.741747
13.886390	1060.909262	12.746765
13.978209	1051.009948	12.751783
13.825805	1064.058580	12.756800
14.010386	1058.360626	12.761818
14.055364	1066.620860	12.766835
14.273285	1076.263333	12.771853
14.091202	1068.106459	12.776871
14.014145	1058.298227	12.781888
14.439855	1066.155438	12.786906
14.377822	1062.532380	12.791923
13.948941	1073.273123	12.796941
14.164428	1069.105656	12.801959
14.109132	1064.183449	12.806976
14.117995	1061.308405	12.811994
14.118696	1059.667203	12.817011
14.033504	1067.272671	12.822029
14.037184	1066.844180	12.827047
14.062092	1065.428864	12.832064
14.316780	1062.947186	12.837082
14.121971	1063.574768	12.842099
14.184884	1072.974784	12.847117
14.313092	1057.251227	12.852135
14.091037	1067.346068	12.857152
14.155751	1064.791272	12.862170
14.514521	1063.361330	12.867187
14.047098	1066.962461	12.872205
14.246828	1060.900048	12.877223
14.319515	1072.352472	12.882240
13.804516	1062.778591	12.887258
14.133500	1064.801874	12.892275
14.329396	1068.365625	12.897293
14.375410	1064.877248	12.902311
14.268681	1063.438613	12.907328
14.312217	1068.475750	12.912346
14.345971	1063.519736	12.917363
13.769454	1065.711352	12.922381
14.093180	1060.112826	12.927399
14.330184	1084.426535	12.932416
14.218326	1102.530938	12.937434
14.564447	1093.860843	12.942451
14.665683	1102.460764	12.947469
14.595329	1088.540789	12.952487
14.632861	1090.267605	12.957504
14.468258	1089.348495	12.962522
14.257123	1092.759270	12.967539
14.033400	1101.564639	12.972557
14.371741	1106.272011	12.977575
14.741765	1090.654303	12.982592
14.446568	1089.406236	12.987610
14.882991	1073.715181	12.992627
14.520924	1094.250723	12.997645
14.380115	1086.230305	13.002663
14.713541	1095.204193	13.007680
14.766706	1096.469635	13.012698
14.486579	1093.383521	13.017715
14.511312	1094.459398	13.022733
14.898781	1094.405216	13.027751
14.639074	1097.284138	13.032768
14.685347	1099.446257	13.037786
14.709967	1090.514771	13.042803
14.418941	1095.352713	13.047821
14.895623	1102.015277	13.052839
14.616872	1095.572736	13.057856
14.501162	1095.971138	13.062874
14.790281	1087.772012	13.067891
14.376262	1095.399161	13.072909
14.865054	1084.348953	13.077927
14.457851	1085.147637	13.082944
14.638029	1083.578136	13.087962
14.869286	1093.058401	13.092979
14.660621	1089.862854	13.097997
14.701360	1092.456925	13.103015
14.904805	1114.171493	13.108032
14.961642	1132.461016	13.113050
15.402640	1115.248714	13.118067
15.102017	1098.995869	13.123085
15.052758	1082.380685	13.128103
15.012806	1084.750919	13.133120
14.786819	1094.120748	13.138138
14.838259	1076.047804	13.143155
14.439130	1087.836633	13.148173
15.056408	1103.854894	13.153191
15.208761	1118.038863	13.158208
15.256386	1108.609149	13.163226
15.071616	1091.160569	13.168243
15.224677	1090.274976	13.173261
15.092722	1088.881052	13.178279
15.115782	1084.221047	13.183296
14.881999	1085.679358	13.188314
14.924431	1077.436763	13.193331
14.746527	1098.578398	13.198349
15.087423	1113.096899	13.203367
15.335046	1107.962638	13.208384
15.329257	1122.197543	13.213402
14.960437	1124.011587	13.218419
15.026016	1120.147184	13.223437
15.368147	1122.298402	13.228455
15.560377	1111.694368	13.233472
15.619964	1112.136429	13.238490
15.298639	1090.662780	13.243507
15.344854	1089.414978	13.248525
15.411905	1087.455767	13.253543
14.915540	1094.500352	13.258560
15.183266	1104.399927	13.263578
15.582092	1107.500885	13.268595
15.343765	1112.660194	13.273613
15.385070	1112.170965	13.278631
15.361043	1117.453106	13.283648
15.216726	1118.883449	13.288666
15.395604	1111.330586	13.293683
15.423273	1120.365840	13.298701
15.389051	1115.963090	13.303719
15.257249	1120.700526	13.308736
15.176389	1123.333001	13.313754
15.404218	1108.104075	13.318771
15.192559	1119.943827	13.323789
15.345101	1125.252297	13.328807
15.570424	1110.638063	13.333824
15.264007	1125.749891	13.338842
15.284356	1120.107199	13.343859
14.983218	1122.450729	13.348877
15.370221	1130.738323	13.353895
15.478896	1132.840142	13.358912
15.436216	1142.524737	13.363930
16.021521	1138.592749	13.368947
15.903724	1138.970437	13.373965
15.635314	1131.808558	13.378983
15.970431	1126.773005	13.384000
15.525589	1129.557741	13.389018
15.354362	1122.448498	13.394035
15.709138	1132.482308	13.399053
15.673916	1138.502617	13.404071
15.780861	1129.862972	13.409088
15.646694	1127.366618	13.414106
15.484473	1138.426476	13.419123
15.303306	1143.831628	13.424141
15.392541	1135.620238	13.429159
15.825235	1129.719666	13.434176
15.758567	1139.164361	13.439194
15.955807	1138.150813	13.444211
15.831776	1136.839815	13.449229
15.931804	1138.681093	13.454247
15.941596	1126.127169	13.459264
15.875574	1135.865413	13.464282
15.784707	1141.253279	13.469299
15.792898	1132.079244	13.474317
15.195126	1130.519612	13.479335
15.791885	1148.043257	13.484352
15.644453	1165.009486	13.489370
16.179984	1163.638502	13.494387
16.200506	1165.686595	13.499405
16.237630	1161.986900	13.504423
16.347964	1162.849060	13.509440
16.136270	1155.968898	13.514458
15.894127	1139.549676	13.519475
16.247339	1148.773635	13.524493
15.872030	1152.463486	13.529511
16.416396	1151.388047	13.534528
16.204855	1149.365826	13.539546
16.229036	1128.691795	13.544563
16.363602	1128.469199	13.549581
16.005794	1131.729443	13.554599
16.148328	1123.569480	13.559616
15.901737	1129.161790	13.564634
16.420923	1149.374836	13.569651
16.391629	1154.685416	13.574669
16.476686	1139.443050	13.579687
16.506588	1131.733916	13.584704
16.055082	1125.206737	13.589722
16.252940	1126.438824	13.594739
16.223429	1128.578042	13.599757
16.174599	1132.627459	13.604775
16.263233	1128.828329	13.609792
16.307311	1147.678952	13.614810
16.831261	1155.904959	13.619827
16.477657	1139.749199	13.624845
16.367782	1135.123546	13.629863
16.783191	1136.962700	13.634880
16.300243	1135.126059	13.639898
16.382141	1133.578699	13.644915
16.639935	1123.534015	13.649933
16.619303	1125.900079	13.654951
16.982984	1118.627652	13.659968
16.617189	1127.624992	13.664986
16.495170	1130.263089	13.670003
16.495937	1126.294057	13.675021
16.548871	1129.817873	13.680039
16.746246	1130.509370	13.685056
16.517152	1128.996279	13.690074
16.889933	1129.250581	13.695091
16.904400	1120.430386	13.700109
16.671878	1126.336466	13.705127
16.650775	1125.280271	13.710144
16.567747	1140.106219	13.715162
16.540351	1131.087059	13.720179
17.051644	1121.586621	13.725197
16.626354	1123.057096	13.730215
17.099148	1114.623696	13.735232
16.534365	1129.564279	13.740250
16.616388	1135.781323	13.745267
16.689343	1123.604701	13.750285
16.462048	1130.180687	13.755303
16.981146	1126.671394	13.760320
16.700903	1125.028389	13.765338
16.234206	1124.019848	13.770355
16.412328	1127.794197	13.775373
16.823277	1144.982850	13.780391
16.988680	1141.305066	13.785408
16.769027	1159.845006	13.790426
16.681741	1156.943712	13.795443
16.859830	1149.952101	13.800461
16.661637	1160.473706	13.805479
17.179504	1153.421221	13.810496
16.940105	1163.066497	13.815514
16.842495	1157.352746	13.820531
16.729302	1158.071750	13.825549
16.815498	1160.829162	13.830567
16.740266	1157.797155	13.835584
16.772620	1157.190523	13.840602
16.831255	1157.167259	13.845619
17.202306	1155.589631	13.850637
16.912211	1168.237740	13.855655
16.677887	1186.100705	13.860672
17.162180	1185.058613	13.865690
17.017190	1188.460841	13.870707
17.438453	1184.296735	13.875725
16.981691	1182.866529	13.880743
17.185047	1183.088012	13.885760
17.286777	1187.760307	13.890778
17.251491	1189.423390	13.895795
17.637770	1179.409202	13.900813
17.330004	1179.379960	13.905831
17.790952	1180.309163	13.910848
17.460538	1182.144226	13.915866
17.261537	1166.209902	13.920883
17.241860	1152.813112	13.925901
17.175316	1178.611177	13.930919
17.552065	1187.810407	13.935936
17.413284	1185.620668	13.940954
17.495768	1189.866874	13.945971
17.738996	1177.398134	13.950989
17.424024	1173.334436	13.956007
17.767731	1162.922824	13.961024
17.493103	1151.815678	13.966042
17.336825	1161.503312	13.971059
17.500534	1158.485749	13.976077
17.113057	1157.064369	13.981095
17.581585	1169.412928	13.986112
17.625124	1171.901840	13.991130
17.603360	1173.437508	13.996147
17.886168	1184.353199	14.001165
17.281454	1176.436556	14.006183
17.544648	1185.890934	14.011200
17.638221	1184.152690	14.016218
17.579656	1189.272083	14.021235
17.968001	1180.583153	14.026253
17.613582	1190.475570	14.031271
17.843906	1188.331908	14.036288
18.269418	1187.277485	14.041306
17.936421	1171.390689	14.046323
18.050941	1153.504249	14.051341
17.189565	1148.880551	14.056359
17.295505	1158.946641	14.061376
17.650752	1161.910541	14.066394
18.081621	1180.098947	14.071411
17.922350	1176.503740	14.076429
17.512564	1184.704364	14.081447
17.720701	1184.998669	14.086464
17.754491	1184.125301	14.091482
17.659143	1181.664840	14.096499
17.910533	1182.281085	14.101517
17.905550	1178.435019	14.106535
17.845742	1180.665460	14.111552
17.841039	1181.802499	14.116570
17.663757	1183.227469	14.121587
17.933186	1184.508158	14.126605
18.010844	1194.475416	14.131623
17.932047	1187.299695	14.136640
18.004735	1182.210850	14.141658
17.669552	1192.861399	14.146675
18.197065	1200.785310	14.151693
17.735731	1213.597561	14.156711
17.749688	1221.457549	14.161728
18.195987	1213.404996	14.166746
18.068413	1213.641211	14.171763
18.158725	1211.754115	14.176781
18.317529	1220.304830	14.181799
18.303100	1218.362610	14.186816
18.239296	1218.692603	14.191834
17.901402	1222.951994	14.196851
17.869503	1213.438324	14.201869
18.087337	1215.902181	14.206887
18.095848	1212.925606	14.211904
18.307775	1204.616554	14.216922
18.176616	1209.011439	14.221939
18.208011	1215.584865	14.226957
18.507953	1220.902470	14.231975
18.417456	1215.863411	14.236992
18.369340	1206.741544	14.242010
18.409541	1220.014743	14.247027
18.835031	1220.586867	14.252045
18.688934	1204.984658	14.257063
18.303416	1205.045615	14.262080
18.483032	1198.924277	14.267098
18.388981	1207.861406	14.272115
18.364325	1200.416926	14.277133
18.390941	1212.639165	14.282151
18.661760	1226.450164	14.287168
19.031660	1220.579616	14.292186
18.771200	1212.182307	14.297203
19.115716	1204.367611	14.302221
18.993684	1207.023239	14.307239
18.664353	1204.350688	14.312256
18.820847	1187.769293	14.317274
18.358197	1206.070940	14.322291
18.506899	1205.112055	14.327309
18.539781	1207.205152	14.332327
18.301390	1197.821074	14.337344
18.822245	1198.338073	14.342362
18.342848	1210.836225	14.347379
18.789773	1221.245165	14.352397
19.044889	1220.353722	14.357415
18.809058	1215.362102	14.362432
19.264769	1215.323608	14.367450
19.043190	1207.188736	14.372467
19.423084	1198.584448	14.377485
18.941509	1189.882793	14.382503
18.808042	1198.412119	14.387520
19.155584	1189.829518	14.392538
18.904504	1192.671604	14.397555
19.103064	1189.344382	14.402573
18.901224	1195.844349	14.407591
18.990329	1198.331443	14.412608
18.918622	1189.002491	14.417626
18.642586	1196.252410	14.422643
19.241285	1200.993154	14.427661
19.275957	1203.555180	14.432679
19.095184	1190.860867	14.437696
19.159378	1186.233005	14.442714
19.102480	1192.325411	14.447731
18.999342	1190.533268	14.452749
19.532672	1203.331121	14.457767
19.556791	1204.066605	14.462784
19.128384	1189.887837	14.467802
18.979219	1192.295030	14.472819
19.206228	1189.132374	14.477837
19.445536	1182.606352	14.482855
19.225087	1184.849758	14.487872
19.389674	1188.140797	14.492890
19.107703	1206.925311	14.497907
19.210684	1197.297249	14.502925
19.248428	1209.520993	14.507943
19.227028	1212.731370	14.512960
19.451427	1216.705151	14.517978
19.370633	1215.099443	14.522995
19.485621	1204.776575	14.528013
19.470915	1214.707739	14.533031
19.360465	1233.218896	14.538048
19.598372	1226.906837	14.543066
19.701887	1227.924239	14.548083
19.526773	1219.378982	14.553101
19.503605	1223.360215	14.558119
19.485687	1229.567045	14.563136
19.623415	1220.740200	14.568154
19.416556	1225.298563	14.573171
19.383264	1224.258547	14.578189
19.667432	1221.981393	14.583207
19.211158	1222.666556	14.588224
19.814242	1218.857774	14.593242
19.620286	1217.229039	14.598259
19.530745	1218.376952	14.603277
19.477325	1219.835583	14.608295
19.322186	1225.884600	14.613312
19.542239	1217.672806	14.618330
19.222195	1233.696708	14.623347
19.621046	1237.092726	14.628365
19.804231	1247.837943	14.633383
19.677041	1255.125883	14.638400
19.994345	1250.048751	14.643418
19.982820	1247.841122	14.648435
19.875988	1253.554457	14.653453
20.398263	1245.882389	14.658471
20.098277	1253.146527	14.663488
20.399701	1246.679298	14.668506
20.105773	1232.357222	14.673523
20.012373	1227.899268	14.678541
20.162836	1210.912011	14.683559
19.821886	1225.522825	14.688576
19.726355	1215.066455	14.693594
19.834562	1241.106772	14.698611
19.842234	1245.763726	14.703629
20.204319	1247.919735	14.708647
20.207058	1254.325101	14.713664
20.116885	1244.340399	14.718682
20.191780	1249.271049	14.723699
19.670884	1252.102819	14.728717
20.162521	1243.129892	14.733735
19.956362	1247.579893	14.738752
20.519517	1241.918511	14.743770
19.854196	1252.641764	14.748787
19.955093	1247.126247	14.753805
20.320989	1240.645020	14.758823
20.480828	1249.539628	14.763840
20.282870	1236.474547	14.768858
20.378153	1248.055239	14.773875
20.255402	1246.708986	14.778893
20.558907	1244.405998	14.783911
20.291239	1257.106372	14.788928
20.209963	1241.913828	14.793946
20.391721	1253.866402	14.798963
20.168029	1268.020931	14.803981
20.681563	1266.595707	14.808999
20.236356	1275.322043	14.814016
20.393151	1265.922218	14.819034
20.549248	1265.216207	14.824051
20.664515	1268.153062	14.829069
20.685016	1270.869979	14.834087
20.899700	1281.930837	14.839104
20.801348	1282.112625	14.844122
21.086121	1270.969834	14.849139
20.732124	1267.485513	14.854157
20.702766	1256.664882	14.859175
20.375273	1252.792773	14.864192
20.992439	1265.514431	14.869210
20.479132	1272.433173	14.874227
20.363284	1276.853300	14.879245
20.992873	1266.297735	14.884263
20.725787	1280.660994	14.889280
20.888718	1268.963417	14.894298
21.323663	1268.264666	14.899315
20.900708	1274.134957	14.904333
20.875401	1260.995071	14.909351
20.373666	1271.378945	14.914368
21.128126	1273.967885	14.919386
21.392904	1269.260401	14.924403
21.082446	1272.344368	14.929421
21.296827	1265.731891	14.934439
20.939799	1263.974805	14.939456
20.918675	1274.722311	14.944474
21.283066	1266.387244	14.949491
21.022841	1266.854407	14.954509
21.053786	1274.110122	14.959527
20.996307	1268.674304	14.964544
20.754142	1264.049019	14.969562
21.323126	1269.919739	14.974579
21.012488	1274.868050	14.979597
21.131389	1266.571778	14.984615
21.064873	1266.238728	14.989632
21.420806	1258.630948	14.994650
21.002858	1270.913314	14.999667
21.239584	1275.302142	15.004685
21.614589	1257.568967	15.009703
21.329759	1266.044810	15.014720
21.439085	1257.304321	15.019738
21.357744	1263.206530	15.024755
21.114390	1263.881900	15.029773
21.210126	1260.777334	15.034791
21.266351	1260.272841	15.039808
21.689182	1264.248682	15.044826
21.387285	1259.770061	15.049843
21.398488	1260.031172	15.054861
21.462750	1264.529589	15.059879
21.376708	1266.738199	15.064896
21.504225	1275.293722	15.069914
21.064741	1260.710672	15.074931
21.451668	1271.681651	15.079949
21.630233	1285.611084	15.084967
21.717770	1292.704327	15.089984
21.796867	1300.812612	15.095002
22.100415	1285.087008	15.100019
21.837901	1269.612815	15.105037
21.214045	1263.317179	15.110055
21.741979	1271.257000	15.115072
21.567850	1282.533861	15.120090
21.762967	1292.700444	15.125107
21.576148	1293.935097	15.130125
21.559361	1281.247858	15.135143
22.171478	1287.309658	15.140160
22.000414	1296.803783	15.145178
22.064967	1294.180875	15.150195
21.622077	1297.800048	15.155213
21.896739	1289.571910	15.160231
21.885774	1300.196315	15.165248
21.851396	1289.347360	15.170266
22.096747	1292.758915	15.175283
21.997406	1290.619919	15.180301
22.077691	1287.383865	15.185319
22.225622	1295.870877	15.190336
22.023206	1290.828835	15.195354
22.449194	1280.162831	15.200371
22.039293	1291.383791	15.205389
22.274021	1283.531102	15.210407
22.484807	1288.729624	15.215424
22.310851	1289.561024	15.220442
22.254782	1260.036315	15.225459
21.955107	1256.961270	15.230477
22.496616	1265.653269	15.235495
22.118284	1265.311322	15.240512
21.952191	1267.911062	15.245530
22.273760	1276.739398	15.250547
22.329001	1272.635950	15.255565
22.408244	1270.659939	15.260583
22.538247	1283.722514	15.265600
22.228999	1284.016897	15.270618
22.460498	1275.329624	15.275635
22.038259	1287.746158	15.280653
22.159742	1269.812573	15.285671
22.114165	1276.249551	15.290688
22.237822	1280.155756	15.295706
22.062175	1286.732327	15.300723
22.218939	1289.470425	15.305741
22.577282	1297.622512	15.310759
22.557407	1296.295863	15.315776
22.307929	1302.110336	15.320794
22.709305	1302.647084	15.325811
22.707876	1309.640091	15.330829
22.916065	1307.958080	15.335847
23.306805	1301.067659	15.340864
22.613342	1285.058052	15.345882
22.694872	1277.709161	15.350899
22.728166	1273.770735	15.355917
22.254210	1277.370434	15.360935
22.620280	1292.268555	15.365952
22.883118	1298.456573	15.370970
23.193774	1300.280385	15.375987
23.107880	1309.263070	15.381005
23.188981	1304.473738	15.386023
22.576053	1280.657385	15.391040
22.415292	1300.312216	15.396058
22.539083	1296.697957	15.401075
22.818880	1309.960377	15.406093
23.150792	1310.756406	15.411111
23.238818	1305.656128	15.416128
23.053451	1308.823157	15.421146
23.192113	1299.222989	15.426163
22.950474	1303.976270	15.431181
22.897739	1310.758691	15.436199
22.800273	1308.640049	15.441216
22.650537	1304.908018	15.446234
23.023099	1306.469864	15.451251
22.716244	1310.136039	15.456269
22.983910	1319.827131	15.461287
23.602675	1330.777358	15.466304
23.501344	1327.834265	15.471322
23.657500	1320.679687	15.476339
23.595138	1312.459992	15.481357
23.595135	1298.203836	15.486375
23.820341	1297.146291	15.491392
23.580233	1300.850247	15.496410
23.789796	1296.769119	15.501427
23.516899	1294.795201	15.506445
23.346613	1295.473653	15.511463
23.575726	1304.403886	15.516480
23.136048	1293.924816	15.521498
23.318383	1289.419113	15.526515
23.299099	1294.513746	15.531533
23.052414	1291.005388	15.536551
23.112043	1292.024536	15.541568
23.274205	1310.448026	15.546586
23.531462	1325.413761	15.551603
23.522240	1330.216230	15.556621
23.804687	1328.648307	15.561639
23.640921	1319.765927	15.566656
23.492320	1329.266398	15.571674
23.918008	1332.104730	15.576691
23.592058	1327.157489	15.581709
23.693228	1331.093206	15.586727
24.041021	1326.919356	15.591744
23.846512	1326.120709	15.596762
24.004709	1335.598435	15.601779
23.628727	1332.646796	15.606797
23.632757	1334.550019	15.611815
23.720301	1325.408419	15.616832
23.550023	1331.800288	15.621850
23.869222	1319.408434	15.626867
23.741627	1328.897955	15.631885
23.747116	1331.453605	15.636903
24.035167	1344.622184	15.641920
23.901905	1356.969960	15.646938
24.279878	1359.883693	15.651955
24.265523	1366.100421	15.656973
24.204910	1357.138383	15.661991
24.702038	1336.683911	15.667008
24.323630	1338.359228	15.672026
24.188789	1337.191319	15.677043
23.958837	1328.052583	15.682061
23.606088	1332.848247	15.687079
24.176051	1339.478574	15.692096
24.481563	1362.461694	15.697114
24.517472	1364.106339	15.702131
24.661331	1367.312271	15.707149
24.585168	1343.733062	15.712167
24.557771	1324.531469	15.717184
24.394637	1327.735177	15.722202
24.357672	1330.029571	15.727219
24.423070	1321.354564	15.732237
24.271154	1326.968303	15.737255
24.675651	1330.418915	15.742272
24.298945	1332.696823	15.747290
24.786938	1339.763869	15.752307
24.607274	1338.742128	15.757325
24.200142	1342.578011	15.762343
24.586056	1342.368989	15.767360
24.560948	1353.741339	15.772378
24.600000	1358.896423	15.777395
24.836357	1357.807508	15.782413
24.440080	1358.239880	15.787431
24.745493	1356.239868	15.792448
25.049510	1361.445840	15.797466
24.807969	1360.319771	15.802483
24.607144	1359.224960	15.807501
24.547084	1356.106953	15.812519
24.789885	1357.662888	15.817536
25.050994	1361.386775	15.822554
25.004343	1353.860040	15.827571
24.842029	1356.137165	15.832589
24.700650	1362.647680	15.837607
24.645645	1349.644104	15.842624
24.704475	1353.146331	15.847642
24.763659	1351.342107	15.852659
24.806406	1363.941475	15.857677
24.667855	1374.121327	15.862695
24.960967	1380.578749	15.867712
25.063740	1381.769294	15.872730
25.099127	1386.113089	15.877747
25.344433	1380.056995	15.882765
25.003092	1381.880699	15.887783
25.182637	1383.515191	15.892800
24.988548	1387.804203	15.897818
25.058692	1391.663775	15.902835
25.351511	1372.157861	15.907853
25.207125	1381.315783	15.912871
25.434115	1374.694090	15.917888
25.409402	1387.060562	15.922906
25.318462	1378.550710	15.927923
25.628654	1384.266233	15.932941
25.363653	1394.185534	15.937959
25.681051	1374.983193	15.942976
25.446392	1378.700635	15.947994
25.422038	1380.659335	15.953011
25.693466	1384.020742	15.958029
25.666232	1384.299032	15.963047
25.490121	1361.348044	15.968064
25.562187	1373.113156	15.973082
25.542684	1381.402913	15.978099
25.611781	1382.712787	15.983117
25.561632	1384.939496	15.988135
25.886152	1371.173276	15.993152
25.455970	1377.475649	15.998170
25.802177	1369.666102	16.003187
25.619439	1369.480585	16.008205
25.614390	1379.096914	16.013223
26.053572	1390.766733	16.018240
25.698321	1385.030322	16.023258
25.541501	1380.574930	16.028275
26.065394	1397.522200	16.033293
25.871702	1405.980500	16.038311
25.828096	1394.157530	16.043328
25.637360	1402.273061	16.048346
25.885007	1399.033733	16.053363
26.224057	1395.069157	16.058381
25.923605	1391.251000	16.063399
26.288460	1403.229923	16.068416
26.132849	1402.668514	16.073434
26.142391	1399.719879	16.078451
26.029201	1388.652804	16.083469
25.932459	1392.752919	16.088487
25.964477	1394.247048	16.093504
25.991439	1401.175571	16.098522
26.129471	1393.487015	16.103539
26.338795	1390.092035	16.108557
25.914163	1399.119528	16.113575
26.046226	1411.610094	16.118592
26.239677	1430.354501	16.123610
26.302950	1429.990946	16.128627
26.998116	1421.922158	16.133645
26.927092	1428.733043	16.138663
26.491919	1405.688202	16.143680
26.558591	1394.130044	16.148698
26.469766	1402.777483	16.153715
26.465837	1391.923817	16.158733
26.385762	1409.267324	16.163751
26.716237	1400.797453	16.168768
26.771416	1419.060625	16.173786
26.254476	1421.276888	16.178803
26.861817	1417.738384	16.183821
26.810834	1426.955298	16.188839
26.382921	1417.726797	16.193856
26.752060	1412.717415	16.198874
26.759310	1425.650414	16.203891
27.018073	1418.297953	16.208909
26.676369	1424.484950	16.213927
26.448061	1417.622177	16.218944
26.651452	1428.306118	16.223962
26.746495	1421.166711	16.228979
27.182693	1419.228533	16.233997
26.856312	1415.242827	16.239015
26.838137	1411.021569	16.244032
27.085803	1411.892147	16.249050
27.080023	1425.159934	16.254067
27.462045	1419.722293	16.259085
27.052218	1419.994918	16.264103
27.185461	1413.199748	16.269120
27.274649	1414.932235	16.274138
27.186323	1425.051859	16.279155
27.635571	1424.659361	16.284173
27.261448	1423.013138	16.289191
27.484354	1408.267149	16.294208
27.237978	1414.779488	16.299226
26.865467	1424.372523	16.304243
27.278832	1416.305822	16.309261
27.196189	1419.721614	16.314279
27.241112	1411.845902	16.319296
27.296355	1416.013612	16.324314
27.090685	1417.801516	16.329331
27.404252	1415.543095	16.334349
27.538584	1425.871367	16.339367
27.182679	1418.256942	16.344384
27.428403	1420.798497	16.349402
27.349139	1419.731816	16.354419
27.346125	1420.855801	16.359437
27.648894	1442.913627	16.364455
27.731921	1448.253576	16.369472
28.145870	1435.486962	16.374490
27.272180	1425.261388	16.379507
27.956158	1429.059292	16.384525
27.662449	1437.291452	16.389543
27.628688	1440.457862	16.394560
27.828083	1434.292419	16.399578
27.947986	1440.711371	16.404595
27.791536	1431.236453	16.409613
27.676413	1427.868704	16.414631
27.649415	1431.287703	16.419648
27.944959	1434.703987	16.424666
27.629492	1435.496779	16.429683
28.044732	1429.046095	16.434701
27.922334	1434.791001	16.439719
27.995272	1430.919597	16.444736
28.323797	1434.636495	16.449754
28.156576	1442.435011	16.454771
27.827505	1432.977398	16.459789
28.163950	1438.693131	16.464807
28.003759	1437.431778	16.469824
28.044723	1438.734693	16.474842
28.147704	1436.433126	16.479859
28.060842	1426.515662	16.484877
28.185651	1444.591200	16.489895
28.210126	1450.516345	16.494912
28.581074	1459.315960	16.499930
28.629918	1461.407438	16.504947
28.690499	1448.259694	16.509965
28.548645	1437.349271	16.514983
28.150322	1432.915467	16.520000
28.637275	1430.440620	16.525018
28.364593	1445.308830	16.530035
28.689502	1449.097187	16.535053
28.755953	1455.690706	16.540071
28.749850	1437.631767	16.545088
28.681213	1421.098739	16.550106
28.433052	1420.768147	16.555123
28.358858	1429.200415	16.560141
28.615452	1441.364560	16.565159
28.417598	1464.396962	16.570176
28.977935	1455.093703	16.575194
28.955360	1462.308948	16.580211
28.630158	1467.668140	16.585229
28.797150	1457.146770	16.590247
28.965704	1458.896262	16.595264
29.138896	1459.980306	16.600282
28.878747	1461.268226	16.605299
28.795040	1459.932822	16.610317
28.850284	1459.643812	16.615335
28.710979	1449.644460	16.620352
28.927351	1456.254539	16.625370
29.231390	1456.031097	16.630387
28.931202	1458.487300	16.635405
28.819944	1458.807229	16.640423
28.874888	1464.700181	16.645440
29.139706	1452.314649	16.650458
28.975100	1460.287130	16.655475
29.360441	1448.553057	16.660493
28.942010	1456.447417	16.665511
29.227494	1456.656909	16.670528
29.463766	1469.706018	16.675546
29.328224	1481.364985	16.680563
29.505520	1484.504794	16.685581
29.568072	1471.871799	16.690599
29.308233	1462.189367	16.695616
29.880199	1463.269318	16.700634
29.645070	1468.961615	16.705651
29.405325	1449.832156	16.710669
29.386849	1443.838915	16.715687
29.495211	1450.565647	16.720704
30.263733	1464.683741	16.725722
29.787448	1460.962725	16.730739
29.369417	1453.294974	16.735757
29.663264	1449.742330	16.740775
29.620543	1444.212488	16.745792
29.859244	1442.447280	16.750810
29.656357	1459.102564	16.755827
29.822834	1464.317522	16.760845
29.972898	1468.311920	16.765863
29.851300	1477.615721	16.770880
29.974328	1467.211832	16.775898
29.837418	1478.398837	16.780915
29.687086	1474.605256	16.785933
29.933437	1471.430096	16.790951
29.641559	1474.655700	16.795968
29.866811	1471.631055	16.800986
29.819842	1470.947963	16.806003
29.943928	1470.395050	16.811021
30.062028	1463.322079	16.816039
29.769847	1474.960672	16.821056
30.124329	1477.533471	16.826074
30.122474	1474.991576	16.831091
29.875029	1493.617602	16.836109
30.454590	1494.646503	16.841127
30.514364	1504.359075	16.846144
30.734807	1488.577912	16.851162
30.637453	1477.692582	16.856179
30.675313	1468.111328	16.861197
30.679824	1454.649655	16.866215
30.199759	1457.291075	16.871232
30.303729	1467.810393	16.876250
30.184933	1464.277910	16.881267
30.559267	1462.863075	16.886285
30.348359	1456.990397	16.891303
30.499213	1479.195806	16.896320
30.803035	1484.077876	16.901338
30.624746	1497.189609	16.906355
30.628527	1501.061159	16.911373
30.722030	1490.849905	16.916391
30.937424	1484.946332	16.921408
31.094556	1481.733164	16.926426
30.944373	1475.803599	16.931443
30.758456	1461.654972	16.936461
30.887118	1462.760940	16.941479
30.387740	1465.391775	16.946496
30.896368	1480.992024	16.951514
30.948414	1489.687091	16.956531
30.888345	1493.579228	16.961549
31.090840	1485.266269	16.966567
30.855253	1496.742002	16.971584
30.870879	1493.166829	16.976602
31.257424	1487.888043	16.981619
31.026496	1501.530462	16.986637
31.121524	1495.372202	16.991655
30.894084	1480.822398	16.996672
31.029419	1494.407436	17.001690
30.901577	1491.217344	17.006707
31.315463	1497.329308	17.011725
30.758666	1492.778383	17.016743
30.790883	1518.472913	17.021760
31.355220	1521.575344	17.026778
31.342824	1537.548525	17.031795
31.301931	1534.975083	17.036813
31.606333	1535.799290	17.041831
31.427596	1526.997404	17.046848
31.399359	1522.748254	17.051866
31.436327	1523.744787	17.056883
31.211802	1533.730315	17.061901
31.555888	1534.241504	17.066919
31.343715	1535.692938	17.071936
31.724145	1536.819505	17.076954
32.176661	1544.538692	17.081971
31.949532	1541.287447	17.086989
31.937658	1521.153625	17.092007
32.032048	1515.643811	17.097024
31.883815	1509.621993	17.102042
32.004359	1510.302389	17.107059
31.610394	1509.432963	17.112077
32.077412	1500.270477	17.117095
32.000543	1516.570984	17.122112
32.293140	1514.918501	17.127130
32.225790	1507.251822	17.132147
32.114478	1506.695882	17.137165
32.430597	1504.722622	17.142183
31.978122	1515.504573	17.147200
31.909585	1509.318816	17.152218
32.110159	1506.145308	17.157235
31.880451	1508.711118	17.162253
32.230223	1504.109189	17.167271
31.969508	1510.383612	17.172288
32.140084	1531.345829	17.177306
32.578150	1533.597578	17.182323
32.737403	1538.307910	17.187341
32.848264	1532.342862	17.192359
32.341522	1525.123147	17.197376
32.034777	1513.960423	17.202394
32.424091	1528.353616	17.207411
32.461473	1533.813722	17.212429
32.647545	1536.388773	17.217447
32.820348	1540.932122	17.222464
32.620684	1538.064876	17.227482
32.874635	1538.016028	17.232499
32.509860	1539.688326	17.237517
32.971853	1537.506727	17.242535
32.968465	1542.695457	17.247552
32.820408	1528.132490	17.252570
32.925789	1505.972072	17.257587
32.813673	1503.132683	17.262605
32.843465	1500.048217	17.267623
32.376001	1503.314455	17.272640
32.692045	1519.591174	17.277658
32.821961	1523.253129	17.282675
32.548802	1532.790448	17.287693
33.017329	1531.208093	17.292711
32.592086	1547.181010	17.297728
32.678034	1531.873352	17.302746
32.803095	1537.482534	17.307763
32.827816	1563.717881	17.312781
33.187409	1556.646886	17.317799
33.308726	1566.976026	17.322816
33.451565	1563.148543	17.327834
33.539370	1564.754913	17.332851
33.209664	1561.651504	17.337869
33.532689	1556.534748	17.342887
33.724497	1563.147358	17.347904
33.425311	1560.891562	17.352922
33.782144	1560.550943	17.357939
33.297350	1555.388368	17.362957
33.655990	1550.400950	17.367975
33.747435	1562.082109	17.372992
33.517893	1558.665924	17.378010
33.648812	1553.490767	17.383027
33.639618	1553.796194	17.388045
33.622868	1553.139794	17.393063
33.489848	1567.973627	17.398080
33.602651	1560.975101	17.403098
33.692823	1558.677600	17.408115
33.735351	1559.840520	17.413133
33.708386	1557.480692	17.418151
33.475146	1559.985487	17.423168
33.759297	1560.316840	17.428186
33.545313	1566.417835	17.433203
33.467488	1571.120902	17.438221
33.748596	1582.108409	17.443239
33.813498	1588.188718	17.448256
33.557948	1598.405569	17.453274
33.928290	1590.642508	17.458291
34.020010	1596.497941	17.463309
33.897693	1584.297325	17.468327
34.148875	1590.038030	17.473344
33.760802	1603.461259	17.478362
34.489452	1608.341467	17.483379
34.425861	1619.476503	17.488397
34.582376	1606.701900	17.493415
34.502381	1608.011434	17.498432
34.246709	1610.457155	17.503450
34.529446	1604.978777	17.508467
34.406629	1613.260537	17.513485
34.943628	1609.121086	17.518503
34.862029	1603.951310	17.523520
34.536955	1597.325878	17.528538
34.635888	1585.254036	17.533555
34.613153	1595.893777	17.538573
35.055008	1602.277901	17.543591
34.891910	1581.548392	17.548608
34.210133	1576.392970	17.553626
34.592429	1592.518678	17.558643
34.776146	1605.663978	17.563661
34.850789	1609.396301	17.568679
34.617316	1603.341490	17.573696
34.993048	1606.188524	17.578714
35.217863	1597.155166	17.583731
34.874163	1608.250074	17.588749
35.172646	1600.869902	17.593767
35.206922	1609.128653	17.598784
34.621933	1609.727829	17.603802
35.443121	1596.267284	17.608819
35.206589	1603.119374	17.613837
35.223101	1600.430346	17.618855
35.367490	1594.893739	17.623872
35.616759	1598.127178	17.628890
35.420194	1606.785843	17.633907
34.993099	1609.965716	17.638925
35.275538	1606.532232	17.643943
35.338758	1600.207750	17.648960
35.378818	1603.520835	17.653978
35.544451	1592.841150	17.658995
35.791980	1601.894090	17.664013
35.385412	1594.334597	17.669031
35.395248	1597.305077	17.674048
35.188365	1601.234099	17.679066
35.435046	1598.525341	17.684083
35.489243	1598.555953	17.689101
35.273150	1594.802930	17.694119
35.559616	1606.585935	17.699136
35.423632	1621.453377	17.704154
35.798617	1626.069825	17.709171
35.796978	1628.928047	17.714189
35.596932	1624.406901	17.719207
35.593530	1629.298649	17.724224
35.607490	1636.839200	17.729242
35.765381	1640.436724	17.734259
35.954087	1636.798078	17.739277
36.033259	1642.894946	17.744295
36.444965	1651.695220	17.749312
36.305125	1644.404190	17.754330
36.275104	1629.810009	17.759347
35.843039	1638.607990	17.764365
36.231215	1653.466594	17.769383
36.291933	1657.299053	17.774400
36.402338	1656.164403	17.779418
36.601233	1664.452668	17.784435
36.840240	1654.919546	17.789453
36.887479	1629.220134	17.794471
36.906049	1635.503175	17.799488
36.401428	1631.413809	17.804506
36.550858	1623.650232	17.809523
36.859333	1629.454311	17.814541
36.490674	1627.451297	17.819559
36.607201	1621.177637	17.824576
36.374112	1627.901821	17.829594
36.546385	1617.345221	17.834611
36.516307	1617.474396	17.839629
36.827306	1624.226176	17.844647
36.633032	1626.864684	17.849664
36.638060	1635.530993	17.854682
37.009495	1647.121072	17.859699
37.018443	1643.482998	17.864717
36.871505	1656.810133	17.869735
36.960333	1644.777114	17.874752
37.124806	1657.813841	17.879770
37.228728	1644.866422	17.884787
36.890771	1652.344084	17.889805
36.663162	1647.263375	17.894823
36.906464	1643.314164	17.899840
36.910141	1648.300407	17.904858
36.800387	1652.696015	17.909875
37.163288	1652.717539	17.914893
36.855178	1653.790787	17.919911
36.817750	1663.148106	17.924928
37.307839	1672.505062	17.929946
37.379015	1675.446132	17.934963
37.255168	1678.286373	17.939981
37.332885	1677.678916	17.944999
37.475073	1665.298519	17.950016
37.438020	1676.314853	17.955034
37.577793	1672.683497	17.960051
37.957207	1658.187951	17.965069
37.538809	1672.363215	17.970087
37.780121	1664.749771	17.975104
37.547331	1666.244777	17.980122
37.664498	1662.184726	17.985139
38.058906	1664.107724	17.990157
37.885650	1668.944884	17.995175
38.201666	1667.144831	18.000192
37.912339	1675.392533	18.005210
37.899011	1662.233200	18.010227
37.854751	1672.712593	18.015245
37.881050	1675.240258	18.020263
38.375345	1673.457786	18.025280
38.160828	1668.584726	18.030298
38.085830	1659.454238	18.035315
38.144608	1669.726466	18.040333
38.104310	1687.249322	18.045351
38.771278	1679.979266	18.050368
38.482368	1676.456932	18.055386
38.403920	1665.554765	18.060403
38.462831	1670.852128	18.065421
38.258173	1673.632108	18.070439
38.608648	1674.030645	18.075456
38.563981	1687.672761	18.080474
38.728436	1679.102627	18.085491
38.847857	1669.400302	18.090509
38.133462	1669.413646	18.095527
38.530793	1679.000674	18.100544
38.617626	1686.537081	18.105562
38.854899	1683.136828	18.110579
38.730830	1687.583625	18.115597
38.640144	1683.770688	18.120615
38.986250	1683.789674	18.125632
38.600351	1686.583662	18.130650
38.622614	1689.499356	18.135667
38.832725	1690.661756	18.140685
38.882297	1694.517718	18.145703
39.216717	1685.518357	18.150720
38.793116	1697.069593	18.155738
38.843981	1689.740139	18.160755
39.143464	1678.946751	18.165773
38.980220	1696.613542	18.170791
39.610436	1697.305581	18.175808
39.109053	1714.070695	18.180826
39.403115	1713.401112	18.185843
39.751385	1716.508386	18.190861
39.200953	1700.044439	18.195879
39.558963	1689.347069	18.200896
39.676945	1694.236888	18.205914
39.354364	1683.500430	18.210931
39.337856	1683.432896	18.215949
39.797624	1705.014222	18.220967
39.756516	1708.809983	18.225984
39.592975	1704.652425	18.231002
39.951629	1712.071887	18.236019
39.672202	1699.906785	18.241037
39.403438	1694.494905	18.246055
39.647403	1708.638300	18.251072
39.809806	1723.859443	18.256090
39.602711	1726.192244	18.261107
39.714843	1715.761841	18.266125
39.611861	1718.486843	18.271143
39.876163	1714.862061	18.276160
39.664768	1711.618611	18.281178
39.755559	1716.660356	18.286195
40.073437	1720.316689	18.291213
39.885859	1735.714954	18.296231
39.962810	1728.315627	18.301248
40.207596	1738.989795	18.306266
40.083161	1738.580881	18.311283
40.242820	1732.505539	18.316301
40.209914	1744.873062	18.321319
40.221551	1733.661699	18.326336
40.452327	1726.107243	18.331354
40.777089	1723.472166	18.336371
40.946153	1711.421309	18.341389
40.671413	1722.060856	18.346407
40.492178	1721.635607	18.351424
40.383956	1717.661404	18.356442
40.506346	1727.008886	18.361459
40.568652	1712.525931	18.366477
40.471611	1720.248234	18.371495
40.467164	1719.087879	18.376512
40.615035	1723.236823	18.381530
40.954042	1744.837175	18.386547
40.995802	1746.531677	18.391565
40.878938	1753.423895	18.396583
41.181446	1755.234741	18.401600
41.090062	1755.657089	18.406618
40.607820	1743.096182	18.411635
40.975834	1746.203152	18.416653
40.912847	1754.191469	18.421671
41.100416	1749.739684	18.426688
41.333235	1754.683570	18.431706
41.162451	1756.407683	18.436723
41.424761	1748.168155	18.441741
41.114430	1753.549395	18.446759
41.244179	1738.384081	18.451776
41.325037	1746.067749	18.456794
40.793115	1750.549876	18.461811
41.182793	1756.468721	18.466829
41.449501	1774.022432	18.471847
41.306227	1774.791312	18.476864
41.374976	1785.867398	18.481882
41.423324	1787.124246	18.486899
41.711473	1770.283486	18.491917
41.792944	1773.538195	18.496935
41.507572	1773.874895	18.501952
41.535212	1778.507256	18.506970
41.702583	1796.067762	18.511987
42.113718	1798.436196	18.517005
41.958732	1795.630999	18.522023
42.159589	1802.867153	18.527040
42.709605	1803.543516	18.532058
42.257781	1791.661725	18.537075
42.430666	1768.732175	18.542093
41.943168	1773.992910	18.547111
42.014645	1769.162313	18.552128
42.439030	1785.501128	18.557146
42.449807	1794.364981	18.562163
42.530919	1787.982550	18.567181
42.436034	1778.436620	18.572199
42.307023	1772.548712	18.577216
42.491665	1780.488251	18.582234
42.480798	1790.646490	18.587251
42.950356	1779.907793	18.592269
42.756904	1782.563906	18.597287
42.668463	1763.253361	18.602304
42.870510	1767.733684	18.607322
42.658366	1772.301150	18.612339
42.683619	1765.595119	18.617357
42.050552	1760.408162	18.622375
42.875283	1777.908245	18.627392
42.840764	1788.901015	18.632410
42.795873	1796.199032	18.637427
42.620237	1792.544186	18.642445
43.011544	1795.684124	18.647463
43.132888	1798.982835	18.652480
43.178684	1807.607665	18.657498
42.815610	1801.575766	18.662515
42.555712	1809.133115	18.667533
42.632935	1801.005435	18.672551
43.034677	1807.108311	18.677568
43.261104	1815.377345	18.682586
42.983186	1828.916411	18.687603
43.051913	1824.116957	18.692621
43.107846	1819.292455	18.697639
43.080149	1813.584818	18.702656
43.344210	1818.926277	18.707674
43.258063	1837.504806	18.712691
43.552659	1838.263138	18.717709
43.441567	1849.771310	18.722727
43.774800	1850.220335	18.727744
44.345491	1841.852838	18.732762
43.936037	1853.588055	18.737779
43.815703	1850.462192	18.742797
44.117835	1845.533226	18.747815
43.767943	1828.116408	18.752832
43.763422	1825.477267	18.757850
43.827536	1846.758264	18.762867
43.913064	1845.139964	18.767885
43.993396	1851.714039	18.772903
44.138690	1849.591030	18.777920
44.341615	1841.287651	18.782938
44.170426	1851.892657	18.787955
44.208122	1850.835160	18.792973
44.300657	1849.738485	18.797991
44.128655	1852.029290	18.803008
44.134269	1842.624571	18.808026
44.440357	1847.611295	18.813043
44.277257	1842.461599	18.818061
44.306033	1845.055019	18.823079
44.251745	1841.135644	18.828096
44.804579	1844.553792	18.833114
44.926721	1869.237493	18.838131
44.642163	1860.058255	18.843149
44.958848	1855.991363	18.848167
44.765654	1849.344422	18.853184
44.952666	1843.196806	18.858202
44.837352	1847.417618	18.863219
44.662154	1845.323753	18.868237
44.670203	1861.822383	18.873255
44.983113	1875.565403	18.878272
44.693096	1867.975886	18.883290
44.776220	1870.957141	18.888307
44.793974	1870.841429	18.893325
44.870790	1878.604956	18.898343
44.560669	1875.703738	18.903360
44.776803	1887.798749	18.908378
44.946702	1898.988505	18.913395
44.855671	1893.782792	18.918413
44.750133	1899.101504	18.923431
44.938040	1908.781151	18.928448
45.662392	1916.112726	18.933466
45.998331	1910.559707	18.938483
46.212586	1907.684222	18.943501
46.090735	1895.081156	18.948519
45.866747	1890.540266	18.953536
45.989403	1892.491075	18.958554
45.993818	1878.220267	18.963571
46.197464	1876.147055	18.968589
46.118353	1878.970886	18.973607
46.520964	1876.451647	18.978624
46.243369	1854.491598	18.983642
46.073100	1858.291811	18.988659
45.855167	1843.303914	18.993677
46.014036	1838.116171	18.998695
45.778283	1853.947474	19.003712
46.025569	1867.848364	19.008730
46.569084	1873.621374	19.013747
46.341362	1872.828775	19.018765
46.368053	1869.036746	19.023783
45.719297	1881.234124	19.028800
46.262766	1873.075420	19.033818
46.369603	1884.358058	19.038835
46.102077	1885.644672	19.043853
46.339195	1877.402546	19.048871
46.121662	1882.810224	19.053888
46.308323	1879.107299	19.058906
46.248519	1887.997828	19.063923
46.198893	1902.469614	19.068941
46.650697	1908.782938	19.073959
46.613492	1913.981318	19.078976
46.975029	1918.648302	19.083994
46.873154	1918.096889	19.089011
46.673125	1912.892450	19.094029
46.586707	1911.832429	19.099047
46.586086	1915.055658	19.104064
46.881136	1930.091518	19.109082
47.081686	1944.802882	19.114099
47.362122	1949.525399	19.119117
47.229814	1943.537390	19.124135
46.938327	1938.168544	19.129152
47.615655	1945.484875	19.134170
47.643000	1940.384968	19.139187
47.500515	1941.859172	19.144205
47.753970	1934.006209	19.149223
47.591297	1939.339690	19.154240
47.592049	1931.574152	19.159258
47.599805	1931.652790	19.164275
47.712142	1926.012120	19.169293
47.946779	1923.124605	19.174311
47.640153	1941.010232	19.179328
47.737134	1925.860188	19.184346
47.645004	1930.273039	19.189363
47.599738	1919.999794	19.194381
47.785508	1931.966996	19.199399
47.454294	1930.469123	19.204416
48.082032	1930.191595	19.209434
47.710610	1934.247487	19.214451
47.665226	1927.334575	19.219469
47.873377	1934.348544	19.224487
47.751131	1947.798019	19.229504
48.113707	1953.438768	19.234522
48.014533	1953.885832	19.239539
48.350413	1950.656217	19.244557
48.255395	1957.533500	19.249575
48.393302	1954.835766	19.254592
48.339119	1956.800452	19.259610
48.255884	1963.007347	19.264627
48.509340	1951.653514	19.269645
48.501197	1966.593067	19.274663
48.279163	1977.544326	19.279680
48.891910	1977.393871	19.284698
48.929183	1981.752089	19.289715
48.739881	1978.427576	19.294733
49.154107	1977.411581	19.299751
49.103682	1979.727585	19.304768
49.175594	1976.151660	19.309786
49.055184	1970.907669	19.314803
48.958293	1969.166758	19.319821
49.289829	1972.522104	19.324839
49.094450	1975.858624	19.329856
49.192036	1978.568243	19.334874
49.542388	1972.188092	19.339891
49.123270	1967.680998	19.344909
49.404055	1970.926040	19.349927
49.230325	1978.054900	19.354944
48.938230	1979.648703	19.359962
49.297262	1965.527071	19.364979
49.396037	1968.025487	19.369997
49.356015	1972.399231	19.375015
48.969930	1990.392131	19.380032
49.174549	1981.441408	19.385050
49.584345	1993.502532	19.390067
49.329007	2001.771166	19.395085
49.463545	2002.269367	19.400103
49.418963	1999.868489	19.405120
50.042498	2000.562435	19.410138
49.840320	2003.380643	19.415155
49.681964	2010.762467	19.420173
50.188974	2011.086727	19.425191
50.223142	2025.560331	19.430208
50.068202	2034.447769	19.435226
50.507749	2037.711468	19.440243
50.278847	2033.288661	19.445261
50.662647	2028.737643	19.450279
50.594746	2032.393435	19.455296
50.580604	2015.374231	19.460314
50.856563	1994.433240	19.465331
50.066847	1993.299682	19.470349
50.311361	1986.270538	19.475367
50.468440	2013.713016	19.480384
50.512369	2023.897982	19.485402
50.942540	2023.866861	19.490419
50.853846	2016.387297	19.495437
50.774987	2020.736175	19.500455
50.672725	2021.086909	19.505472
50.805586	2023.490142	19.510490
50.945692	2021.281557	19.515507
50.532907	2016.401388	19.520525
50.887291	2010.917327	19.525543
51.086195	2015.719473	19.530560
51.373774	2017.903849	19.535578
50.915596	2015.293779	19.540595
51.410988	2025.909217	19.545613
51.382645	2020.542132	19.550631
51.390511	2038.592224	19.555648
51.513266	2035.943825	19.560666
51.723506	2040.117192	19.565683
51.831818	2035.169411	19.570701
52.150092	2031.260858	19.575719
51.810329	2007.698602	19.580736
51.835074	1990.946399	19.585754
51.834186	1989.166003	19.590771
51.757848	2002.422720	19.595789
51.840408	1998.943643	19.600807
51.796846	1992.132163	19.605824
51.597922	1987.472153	19.610842
52.127350	1993.614826	19.615859
51.896486	2003.936713	19.620877
51.768101	2004.407698	19.625895
51.997304	2025.672094	19.630912
51.952678	2039.566263	19.635930
52.326067	2023.748651	19.640947
51.734484	2033.292837	19.645965
52.088991	2029.534977	19.650983
52.254648	2029.982174	19.656000
52.116993	2032.405309	19.661018
52.236340	2024.420538	19.666035
52.202251	2046.215239	19.671053
52.431535	2057.812584	19.676071
52.772580	2061.407893	19.681088
52.456080	2069.103254	19.686106
52.939740	2052.315306	19.691123
52.599221	2060.444319	19.696141
52.801756	2058.794263	19.701159
53.064702	2060.119993	19.706176
52.741519	2059.483698	19.711194
53.217166	2051.337683	19.716211
53.011009	2050.315940	19.721229
52.852778	2052.411208	19.726247
53.128782	2064.820257	19.731264
52.791049	2054.725948	19.736282
53.261311	2045.511232	19.741299
53.101584	2071.511804	19.746317
53.204842	2080.905376	19.751335
53.412242	2076.339403	19.756352
53.584973	2077.842825	19.761370
53.454733	2069.667796	19.766387
53.487958	2078.888113	19.771405
53.755849	2073.996816	19.776423
53.717695	2069.491695	19.781440
53.501270	2063.341766	19.786458
53.691299	2055.183896	19.791475
53.461246	2069.363633	19.796493
53.865429	2067.354100	19.801511
53.758422	2068.525431	19.806528
53.888891	2079.013429	19.811546
54.450815	2083.663098	19.816563
54.188397	2098.828837	19.821581
54.420801	2098.702258	19.826599
54.369674	2077.578412	19.831616
54.143005	2071.673262	19.836634
54.541529	2074.102874	19.841651
54.362191	2086.219694	19.846669
54.616721	2089.801355	19.851687
54.412033	2086.549237	19.856704
54.794566	2090.296936	19.861722
54.571220	2090.812156	19.866739
54.465102	2100.819030	19.871757
54.735132	2101.282051	19.876775
54.370125	2088.911115	19.881792
54.433868	2085.623695	19.886810
54.488563	2089.045087	19.891827
54.665564	2092.991106	19.896845
54.754203	2091.441159	19.901863
54.702192	2096.794987	19.906880
54.773152	2116.302537	19.911898
54.833668	2121.404727	19.916915
55.066729	2123.785711	19.921933
55.278374	2123.928682	19.926951
55.188638	2117.069664	19.931968
55.231460	2124.160838	19.936986
55.337988	2113.007529	19.942003
54.970765	2124.677316	19.947021
54.995489	2146.780130	19.952039
55.341961	2148.843386	19.957056
55.602784	2152.756673	19.962074
55.926346	2154.211755	19.967091
55.931528	2144.188075	19.972109
55.752121	2138.588057	19.977127
56.316531	2133.754625	19.982144
56.350146	2144.294693	19.987162
56.129325	2140.026609	19.992179
56.006667	2142.952558	19.997197
56.307749	2133.919670	20.002215
56.110832	2132.256092	20.007232
56.041749	2142.790493	20.012250
56.275122	2142.472430	20.017267
56.072308	2149.426267	20.022285
56.281090	2143.089123	20.027303
56.221181	2140.042382	20.032320
56.078796	2134.353381	20.037338
56.306740	2133.988778	20.042355
56.160755	2150.301179	20.047373
56.264577	2154.705728	20.052391
56.524258	2158.761123	20.057408
56.653100	2171.397513	20.062426
56.636028	2162.952573	20.067443
56.515316	2170.885689	20.072461
56.450423	2171.571366	20.077479
56.951412	2170.232582	20.082496
56.694975	2178.876659	20.087514
56.659352	2174.354161	20.092531
56.685807	2187.151369	20.097549
57.158038	2194.062768	20.102567
57.212063	2191.180838	20.107584
57.073902	2201.048989	20.112602
57.418925	2200.860299	20.117619
57.552440	2197.508377	20.122637
57.313590	2194.459504	20.127655
57.750131	2186.713945	20.132672
57.442905	2188.299246	20.137690
57.418214	2199.671758	20.142707
57.715720	2192.559754	20.147725
57.671677	2198.886636	20.152743
58.034709	2184.459639	20.157760
57.807545	2189.480069	20.162778
57.948215	2185.471112	20.167795
57.856328	2201.279193	20.172813
57.769763	2205.842766	20.177831
58.048695	2205.872068	20.182848
57.839664	2217.787023	20.187866
58.320560	2214.437927	20.192883
58.192624	2213.267627	20.197901
57.875904	2219.688982	20.202919
58.203128	2211.466039	20.207936
58.220915	2218.940106	20.212954
58.348784	2227.008539	20.217971
58.727709	2237.508537	20.222989
58.539457	2244.669641	20.228007
58.975588	2241.687359	20.233024
58.828369	2243.319449	20.238042
58.965809	2234.976093	20.243059
59.196429	2238.518240	20.248077
58.524780	2245.866498	20.253095
58.954125	2228.982028	20.258112
58.988394	2236.622265	20.263130
58.863047	2239.165043	20.268147
59.151587	2234.504913	20.273165
58.967356	2238.434682	20.278183
59.227958	2232.826286	20.283200
59.262460	2231.841136	20.288218
59.132318	2236.875270	20.293235
59.469236	2236.561748	20.298253
59.330588	2222.342606	20.303271
59.416866	2225.011030	20.308288
59.437538	2229.069131	20.313306
59.511616	2237.174409	20.318323
60.094418	2249.362254	20.323341
59.719597	2246.116169	20.328359
60.211668	2233.162381	20.333376
60.067276	2244.830867	20.338394
60.018035	2224.026367	20.343411
60.145743	2226.930644	20.348429
59.667324	2224.084725	20.353447
59.943053	2237.881849	20.358464
59.933922	2247.316533	20.363482
60.273058	2254.784364	20.368499
60.288258	2257.586380	20.373517
60.501958	2257.807945	20.378535
60.367196	2248.519279	20.383552
60.364606	2253.454001	20.388570
60.152201	2249.473845	20.393587
60.252744	2252.166687	20.398605
59.666929	2256.429926	20.403623
60.290185	2273.515477	20.408640
60.582900	2274.626284	20.413658
60.555734	2284.019879	20.418675
60.848214	2280.076357	20.423693
60.623817	2292.036819	20.428711
60.902298	2292.121310	20.433728
60.945391	2301.985360	20.438746
60.830245	2309.117879	20.443763
61.487394	2300.316392	20.448781
61.296440	2308.702100	20.453799
61.446592	2307.514973	20.458816
61.539961	2305.168608	20.463834
61.695774	2301.768297	20.468851
61.810617	2296.799867	20.473869
61.752832	2301.351626	20.478887
62.067986	2297.426202	20.483904
61.950436	2301.835092	20.488922
61.716144	2310.327561	20.493939
62.114635	2306.470248	20.498957
61.949667	2300.941204	20.503975
62.084161	2299.929685	20.508992
61.966032	2303.624941	20.514010
62.000930	2307.449625	20.519027
62.087652	2303.401524	20.524045
61.703477	2292.044349	20.529063
62.024146	2281.989706	20.534080
61.905053	2290.328295	20.539098
61.892676	2283.996736	20.544115
62.187644	2303.336806	20.549133
62.156511	2327.651714	20.554151
62.303519	2322.956484	20.559168
62.095132	2330.068006	20.564186
61.930515	2324.641645	20.569203
62.453193	2341.063425	20.574221
62.635457	2353.915334	20.579239
62.890343	2347.110677	20.584256
62.868026	2354.567422	20.589274
63.216915	2352.994719	20.594291
63.369352	2353.757870	20.599309
63.322127	2362.675332	20.604327
63.498589	2347.404070	20.609344
63.252167	2343.722996	20.614362
63.276104	2346.016138	20.619379
63.434439	2355.028163	20.624397
63.698457	2356.028568	20.629415
63.447705	2347.133197	20.634432
63.590833	2342.907863	20.639450
63.515423	2351.249306	20.644467
63.597849	2350.847528	20.649485
63.446484	2355.572040	20.654503
63.464364	2341.584780	20.659520
63.748475	2333.782452	20.664538
63.420280	2354.392411	20.669555
63.761912	2363.816053	20.674573
63.549495	2377.985874	20.679591
64.046861	2369.438099	20.684608
64.364195	2366.353581	20.689626
64.334125	2373.145912	20.694643
64.659766	2361.930431	20.699661
64.389360	2370.081876	20.704679
64.444359	2362.227438	20.709696
64.568145	2367.260401	20.714714
64.023905	2361.969783	20.719731
64.861223	2365.342027	20.724749
64.569182	2366.176066	20.729767
64.598829	2368.092702	20.734784
64.588994	2366.501524	20.739802
64.899536	2367.344645	20.744819
64.802048	2369.675964	20.749837
64.836399	2394.380524	20.754855
64.761531	2403.172664	20.759872
64.924680	2394.391538	20.764890
64.913258	2400.615086	20.769907
64.909581	2398.924074	20.774925
65.016075	2401.515768	20.779943
65.151958	2405.406068	20.784960
65.454194	2418.834429	20.789978
65.192947	2429.336412	20.794995
65.627937	2426.199372	20.800013
65.691960	2430.132259	20.805031
65.470148	2422.572926	20.810048
65.855268	2426.894852	20.815066
65.328068	2427.286286	20.820083
65.961651	2418.574645	20.825101
65.936586	2427.967194	20.830119
65.887133	2421.482855	20.835136
65.909689	2432.235170	20.840154
65.945121	2446.708764	20.845171
66.204886	2440.157575	20.850189
66.326295	2442.746811	20.855207
65.951056	2446.158228	20.860224
66.427327	2433.624379	20.865242
65.858521	2438.176767	20.870259
66.033859	2448.799917	20.875277
66.517385	2461.233455	20.880295
66.824456	2467.341020	20.885312
67.073274	2470.058805	20.890330
67.033251	2469.334759	20.895347
67.270106	2464.720304	20.900365
67.125164	2468.937322	20.905383
67.301496	2461.825141	20.910400
67.351563	2467.491344	20.915418
67.433405	2465.111430	20.920435
67.778093	2451.777704	20.925453
67.852821	2442.993051	20.930471
67.477812	2430.774665	20.935488
67.351880	2418.919042	20.940506
67.297332	2437.020658	20.945523
67.339646	2429.930244	20.950541
67.357406	2449.221822	20.955559
67.458309	2451.695557	20.960576
67.641548	2453.530922	20.965594
67.327803	2461.783075	20.970611
67.474694	2458.224764	20.975629
67.363674	2458.463181	20.980647
67.293901	2478.629839	20.985664
67.459266	2483.042422	20.990682
67.356155	2485.935285	20.995699
67.949169	2489.377650	21.000717
68.030412	2503.500045	21.005735
68.059129	2523.375305	21.010752
68.117987	2521.131456	21.015770
68.056189	2513.939316	21.020787
68.761753	2515.523032	21.025805
68.659762	2514.171857	21.030823
68.450585	2514.512710	21.035840
68.897300	2510.490301	21.040858
68.798043	2534.276269	21.045875
69.396927	2533.286812	21.050893
69.196667	2514.387089	21.055911
69.103040	2506.727796	21.060928
69.306219	2501.905127	21.065946
68.992724	2511.363890	21.070963
69.074329	2520.801070	21.075981
69.243783	2518.066925	21.080999
69.342599	2531.660881	21.086016
69.501058	2532.537804	21.091034
69.307683	2538.848164	21.096051
69.247926	2537.156168	21.101069
69.516098	2523.601966	21.106087
69.435674	2532.536035	21.111104
69.898523	2526.986628	21.116122
69.526626	2529.459767	21.121139
69.336915	2547.087023	21.126157
69.687059	2552.224564	21.131175
69.763312	2558.951378	21.136192
69.850137	2556.979660	21.141210
70.077530	2557.796377	21.146227
70.059526	2558.399326	21.151245
69.998513	2577.702506	21.156263
70.335870	2585.031822	21.161280
70.758109	2583.414104	21.166298
70.683122	2578.700365	21.171315
70.887546	2571.993314	21.176333
71.185932	2584.906341	21.181351
70.944650	2584.558442	21.186368
71.147571	2579.174796	21.191386
71.366137	2580.637428	21.196403
71.153441	2574.847683	21.201421
71.235527	2565.736171	21.206439
70.895239	2574.095126	21.211456
71.219660	2574.932424	21.216474
71.006620	2578.893809	21.221491
71.524734	2567.267852	21.226509
71.383302	2571.571715	21.231527
71.211839	2581.596784	21.236544
71.513305	2577.432620	21.241562
71.308213	2579.535307	21.246579
71.330735	2567.744011	21.251597
71.500432	2581.192840	21.256615
71.448553	2603.205428	21.261632
71.580270	2607.051194	21.266650
71.900108	2618.334013	21.271667
71.551962	2612.818985	21.276685
71.528653	2613.820826	21.281703
71.613135	2632.586671	21.286720
72.036355	2636.488208	21.291738
72.620507	2640.334415	21.296755
72.513823	2633.679926	21.301773
72.931909	2624.995906	21.306791
72.786501	2635.958785	21.311808
72.820310	2623.933309	21.316826
72.859474	2637.212033	21.321843
72.811304	2630.371507	21.326861
72.911151	2620.447225	21.331879
72.982908	2631.443111	21.336896
73.096548	2623.216860	21.341914
72.958188	2634.319905	21.346931
72.936891	2621.772065	21.351949
73.126965	2614.852023	21.356967
73.062111	2632.654405	21.361984
72.949187	2621.768871	21.367002
73.220237	2624.867243	21.372019
73.002079	2634.033962	21.377037
73.217104	2645.639225	21.382055
73.070665	2646.388985	21.387072
73.424145	2649.985135	21.392090
73.215153	2655.129281	21.397107
73.494851	2680.769695	21.402125
73.596708	2683.076782	21.407143
73.531387	2685.675262	21.412160
73.930771	2684.963633	21.417178
73.821193	2689.374071	21.422195
74.115331	2684.227274	21.427213
74.058538	2687.270389	21.432231
73.771004	2707.029252	21.437248
74.491998	2710.093448	21.442266
74.323907	2710.549164	21.447283
74.272297	2722.924104	21.452301
74.741389	2711.755334	21.457319
74.660298	2714.058012	21.462336
74.957500	2709.045341	21.467354
74.740374	2709.006425	21.472371
74.765983	2712.269776	21.477389
75.333962	2728.542562	21.482407
75.039075	2739.388488	21.487424
75.355709	2731.985295	21.492442
75.550870	2730.409809	21.497459
75.401762	2733.291422	21.502477
75.881527	2715.184560	21.507495
75.672832	2715.417468	21.512512
75.139490	2708.835810	21.517530
75.625253	2722.059314	21.522547
75.919868	2726.378565	21.527565
76.116157	2709.091354	21.532583
75.926311	2725.320864	21.537600
76.079351	2717.550632	21.542618
75.942557	2717.686623	21.547635
75.722729	2723.010919	21.552653
75.929286	2722.947661	21.557671
76.131188	2727.073186	21.562688
76.536890	2714.252754	21.567706
76.263643	2712.358230	21.572723
75.998173	2713.001684	21.577741
76.319607	2733.337484	21.582759
76.405887	2754.156639	21.587776
76.342992	2741.618726	21.592794
76.804914	2751.823878	21.597811
76.521609	2760.075488	21.602829
76.476026	2751.861701	21.607847
76.687004	2770.879636	21.612864
76.938467	2774.385197	21.617882
76.911405	2777.889933	21.622899
76.814354	2786.551709	21.627917
76.987203	2780.913131	21.632935
77.023674	2782.678303	21.637952
77.387765	2793.761820	21.642970
77.762535	2794.713247	21.647987
77.795090	2812.915079	21.653005
77.666125	2800.867545	21.658023
77.780593	2804.757941	21.663040
78.007394	2807.123532	21.668058
78.096790	2800.626328	21.673075
78.048484	2803.538146	21.678093
78.005503	2804.746391	21.683111
78.133600	2815.357521	21.688128
77.896697	2796.265484	21.693146
78.140382	2807.103956	21.698163
78.108362	2798.070610	21.703181
78.289899	2792.318785	21.708199
78.080858	2804.846964	21.713216
78.215866	2806.577747	21.718234
78.746091	2803.687879	21.723251
78.633370	2823.360132	21.728269
79.005517	2827.335510	21.733287
78.858895	2832.172567	21.738304
78.900955	2825.470583	21.743322
78.944129	2828.537362	21.748339
78.467438	2828.399609	21.753357
78.823901	2815.400622	21.758375
78.721202	2834.527946	21.763392
78.780545	2844.922512	21.768410
78.983667	2852.615071	21.773427
78.792790	2855.761868	21.778445
79.101944	2873.070455	21.783463
79.675962	2874.485798	21.788480
79.709518	2875.895568	21.793498
80.055268	2879.132432	21.798515
79.766775	2879.959611	21.803533
79.723383	2872.879219	21.808551
80.011368	2875.797291	21.813568
80.284317	2876.038013	21.818586
80.506621	2868.673176	21.823603
80.382737	2861.973007	21.828621
80.487089	2860.824311	21.833639
80.790314	2861.977322	21.838656
80.466707	2860.946191	21.843674
80.845936	2878.704214	21.848691
80.823027	2894.056343	21.853709
81.001837	2888.304146	21.858727
81.171852	2894.285714	21.863744
80.897142	2899.051441	21.868762
81.184364	2886.579568	21.873779
81.151176	2894.591896	21.878797
81.294591	2881.997731	21.883815
81.059243	2893.640200	21.888832
81.243216	2894.068453	21.893850
81.662557	2892.110643	21.898867
81.431834	2889.743337	21.903885
81.416591	2881.704776	21.908903
81.759562	2893.613483	21.913920
81.337406	2890.719559	21.918938
81.775826	2890.089264	21.923955
81.661259	2911.600066	21.928973
81.818882	2917.580541	21.933991
81.858196	2915.040661	21.939008
81.488003	2923.165381	21.944026
81.955122	2912.152302	21.949043
82.072937	2944.075624	21.954061
82.264183	2940.806323	21.959079
82.589486	2947.024056	21.964096
82.320515	2951.683735	21.969114
82.216306	2941.904380	21.974131
82.485209	2942.869767	21.979149
82.930179	2954.599073	21.984167
83.039626	2963.556344	21.989184
82.906974	2967.591550	21.994202
83.057697	2967.478070	21.999219
83.101399	2971.020763	22.004237
83.223492	2964.636981	22.009255
83.477535	2964.567451	22.014272
83.606210	2969.854324	22.019290
83.748005	2966.719564	22.024307
83.626851	2976.883814	22.029325
83.781531	2962.502730	22.034343
83.844172	2958.354700	22.039360
83.846014	2968.987979	22.044378
83.999946	2966.878746	22.049395
84.342863	2976.012401	22.054413
84.073260	2960.938454	22.059431
84.199747	2960.628590	22.064448
84.100024	2957.736491	22.069466
84.251208	2961.064969	22.074483
84.001609	2961.513295	22.079501
84.084433	2957.021388	22.084519
84.118041	2972.037886	22.089536
84.168831	2992.531345	22.094554
84.147879	2987.731388	22.099571
84.284912	2990.539783	22.104589
84.676402	2995.462773	22.109607
84.835056	3006.887469	22.114624
84.730850	3023.518484	22.119642
84.983378	3022.883862	22.124659
84.980113	3023.750136	22.129677
85.147433	3023.318567	22.134695
85.306041	3017.307855	22.139712
85.491656	3041.354609	22.144730
85.515408	3052.209123	22.149747
85.699885	3042.652075	22.154765
85.716662	3040.522583	22.159783
85.763230	3043.859704	22.164800
85.537854	3055.980557	22.169818
85.802683	3046.258264	22.174835
85.861906	3046.017781	22.179853
86.040690	3058.454522	22.184871
86.204280	3063.357319	22.189888
86.082753	3067.719445	22.194906
86.286389	3069.237347	22.199923
86.136200	3077.560435	22.204941
86.054410	3074.230319	22.209959
86.415946	3078.077597	22.214976
86.388526	3095.171582	22.219994
86.627800	3105.074001	22.225011
86.907353	3106.146693	22.230029
86.785206	3102.853948	22.235047
86.842703	3099.499630	22.240064
86.928413	3121.829976	22.245082
86.907721	3127.456933	22.250099
86.901006	3130.366664	22.255117
87.176741	3130.222291	22.260135
87.540176	3133.105111	22.265152
87.417582	3159.451366	22.270170
87.902063	3157.805591	22.275187
88.329886	3155.114468	22.280205
88.157527	3160.105878	22.285223
88.122858	3149.672390	22.290240
88.234038	3159.827897	22.295258
88.334230	3156.714540	22.300275
88.125664	3149.725881	22.305293
88.380876	3151.399046	22.310311
88.634651	3134.878623	22.315328
88.811070	3140.400574	22.320346
88.847846	3138.525241	22.325363
89.121422	3138.791848	22.330381
88.925381	3141.469089	22.335399
89.149913	3129.474304	22.340416
89.061957	3140.576862	22.345434
89.217396	3131.416678	22.350451
89.266779	3131.128607	22.355469
89.137756	3136.660478	22.360487
89.563429	3121.000628	22.365504
89.230464	3134.757405	22.370522
89.362755	3124.387682	22.375539
89.315910	3126.990663	22.380557
89.144860	3128.086239	22.385575
89.464571	3130.384167	22.390592
89.105238	3135.079698	22.395610
89.659898	3141.371026	22.400627
89.329657	3152.910473	22.405645
89.421632	3162.249088	22.410663
89.669585	3177.468552	22.415680
89.856195	3190.466698	22.420698
90.003389	3195.711218	22.425715
90.294220	3197.528107	22.430733
89.959536	3209.432105	22.435751
90.087861	3219.711982	22.440768
90.017959	3221.602260	22.445786
90.706678	3214.794436	22.450803
91.442399	3211.574086	22.455821
91.140757	3206.513753	22.460839
91.255472	3203.996406	22.465856
91.035773	3211.004687	22.470874
91.075574	3212.822901	22.475891
91.346498	3221.251676	22.480909
91.054983	3240.632745	22.485927
91.370434	3235.704685	22.490944
90.954561	3235.666717	22.495962
91.171174	3240.446636	22.500979
91.719921	3259.209755	22.505997
91.718426	3262.803682	22.511015
91.919766	3257.626363	22.516032
91.527736	3271.430814	22.521050
91.790989	3276.842798	22.526067
92.477456	3283.325003	22.531085
92.496709	3294.314287	22.536103
92.448907	3290.089930	22.541120
92.620730	3294.306404	22.546138
92.796623	3298.084414	22.551155
92.982709	3292.467086	22.556173
92.783738	3290.982654	22.561191
93.120833	3279.047500	22.566208
93.099308	3285.936456	22.571226
92.954028	3282.993555	22.576243
93.343364	3282.617813	22.581261
93.159314	3285.898606	22.586279
93.334444	3276.193354	22.591296
93.326547	3289.169392	22.596314
93.763037	3290.556714	22.601331
93.956635	3293.610935	22.606349
93.988545	3307.066235	22.611367
93.905938	3306.559420	22.616384
93.857606	3304.730019	22.621402
93.914008	3309.405331	22.626419
94.271282	3298.409343	22.631437
93.801766	3306.749098	22.636455
94.438430	3297.035680	22.641472
94.091341	3300.349716	22.646490
94.432829	3325.368394	22.651507
94.570129	3324.919730	22.656525
94.315818	3332.801892	22.661543
94.835309	3327.794813	22.666560
95.208380	3321.512721	22.671578
95.021766	3316.899484	22.676595
95.570353	3320.327728	22.681613
95.147227	3323.624412	22.686631
95.342277	3312.385142	22.691648
95.173678	3324.400366	22.696666
95.063119	3324.548561	22.701683
95.625751	3321.975686	22.706701
95.275291	3324.663908	22.711719
95.409656	3325.799189	22.716736
95.414662	3341.823523	22.721754
95.424702	3355.314368	22.726771
95.527686	3351.796575	22.731789
95.729459	3354.562843	22.736807
96.256051	3368.404172	22.741824
96.182167	3382.688829	22.746842
96.167756	3388.029409	22.751859
96.260909	3373.306930	22.756877
96.253356	3381.943226	22.761895
96.449553	3371.514747	22.766912
96.482018	3384.131046	22.771930
96.625270	3401.085749	22.776947
97.262499	3404.538341	22.781965
96.893278	3406.364321	22.786983
97.153470	3398.283130	22.792000
97.024214	3408.297426	22.797018
97.172731	3406.453990	22.802035
97.612036	3409.638107	22.807053
96.907821	3410.391091	22.812071
97.412475	3418.645527	22.817088
97.455751	3432.069923	22.822106
97.430933	3438.216967	22.827123
97.646099	3434.382586	22.832141
97.378529	3447.385522	22.837159
97.630701	3463.872293	22.842176
97.897170	3462.516056	22.847194
97.586636	3469.954426	22.852211
98.535654	3470.496836	22.857229
98.606734	3487.630095	22.862247
98.944575	3493.361722	22.867264
98.972702	3486.769236	22.872282
98.888040	3474.093775	22.877299
98.990635	3481.990661	22.882317
99.121875	3490.411562	22.887335
99.522207	3492.177716	22.892352
99.254911	3478.343049	22.897370
99.130023	3487.466118	22.902387
99.409430	3474.786797	22.907405
99.222840	3491.136254	22.912423
99.624412	3478.291467	22.917440
99.767654	3487.308813	22.922458
99.583848	3498.167620	22.927475
99.816781	3508.159142	22.932493
99.917577	3512.417334	22.937511
100.103900	3522.048846	22.942528
99.992219	3514.660938	22.947546
99.537577	3513.489600	22.952563
100.029112	3527.945925	22.957581
99.777925	3550.816026	22.962599
100.334087	3546.612276	22.967616
100.249482	3551.673957	22.972634
100.704158	3570.415596	22.977651
100.949632	3574.777066	22.982669
100.826172	3574.412821	22.987687
100.806710	3571.807348	22.992704
100.479818	3579.514224	22.997722
100.676547	3589.613357	23.002739
101.615020	3590.244524	23.007757
101.441220	3591.031527	23.012775
101.376226	3591.844252	23.017792
101.919065	3583.960753	23.022810
101.588173	3597.405779	23.027827
101.999440	3594.072034	23.032845
101.984510	3589.056327	23.037863
102.440696	3591.830600	23.042880
102.479308	3579.220117	23.047898
102.088736	3591.732861	23.052915
102.451790	3590.787038	23.057933
102.466413	3604.019464	23.062951
102.697780	3602.703269	23.067968
102.902923	3616.610534	23.072986
102.612529	3617.073491	23.078003
102.731690	3608.787145	23.083021
102.491266	3604.522876	23.088039
102.806828	3612.190935	23.093056
102.742325	3608.121223	23.098074
102.707389	3633.417167	23.103091
103.033268	3638.505932	23.108109
103.302469	3634.934232	23.113127
103.166284	3642.706873	23.118144
103.495086	3665.968717	23.123162
103.377703	3661.803789	23.128179
103.743169	3663.574150	23.133197
103.914741	3667.869509	23.138215
104.124836	3671.729756	23.143232
103.993021	3683.384841	23.148250
104.182453	3691.497018	23.153267
104.539723	3704.732361	23.158285
104.395923	3696.984311	23.163303
104.306039	3688.396631	23.168320
104.610529	3697.887465	23.173338
104.941657	3702.350175	23.178355
105.037119	3708.964076	23.183373
105.133962	3724.946465	23.188391
105.216962	3717.975120	23.193408
105.716158	3717.030811	23.198426
105.361773	3724.361190	23.203443
105.427070	3719.702665	23.208461
105.319675	3712.180881	23.213479
105.096420	3706.087723	23.218496
105.349867	3720.342226	23.223514
105.591939	3743.874823	23.228531
105.944228	3744.927669	23.233549
105.827881	3742.374791	23.238567
106.233693	3743.501472	23.243584
106.405272	3752.883196	23.248602
106.732415	3765.299928	23.253619
106.657387	3752.663199	23.258637
106.909641	3760.771331	23.263655
107.108984	3764.695190	23.268672
107.503700	3747.942556	23.273690
107.325847	3757.089495	23.278707
107.776613	3751.227082	23.283725
107.378493	3733.458590	23.288743
107.117801	3730.925628	23.293760
107.549145	3741.757765	23.298778
107.229329	3749.226542	23.303795
107.434133	3744.556769	23.308813
107.854969	3751.575597	23.313831
107.899487	3765.987896	23.318848
107.936551	3752.859799	23.323866
107.459250	3763.385781	23.328883
107.500705	3770.979129	23.333901
107.636188	3776.484844	23.338919
107.928197	3775.927925	23.343936
107.945750	3798.090580	23.348954
107.976210	3819.478672	23.353971
108.291312	3816.083997	23.358989
108.734405	3815.167063	23.364007
108.514156	3831.249989	23.369024
108.968661	3842.011044	23.374042
108.991348	3846.845243	23.379059
108.870729	3844.395420	23.384077
109.254947	3845.146925	23.389095
109.000279	3838.894333	23.394112
109.452689	3839.779457	23.399130
109.089229	3864.667448	23.404147
109.522270	3875.163560	23.409165
109.600801	3867.964140	23.414183
109.498535	3870.811449	23.419200
109.900882	3878.157023	23.424218
110.031596	3894.709992	23.429235
110.380862	3891.443913	23.434253
110.360711	3886.062031	23.439271
110.134357	3888.791653	23.444288
110.674920	3890.131127	23.449306
110.706638	3890.833002	23.454323
111.027526	3903.189065	23.459341
111.213143	3922.188194	23.464359
111.203483	3918.098708	23.469376
111.368114	3913.824513	23.474394
111.012062	3917.931524	23.479411
111.387960	3913.152719	23.484429
111.647667	3908.387208	23.489447
111.380493	3912.163773	23.494464
111.493339	3906.133509	23.499482
111.616051	3919.851904	23.504499
112.059827	3923.962195	23.509517
111.924788	3941.128437	23.514535
111.543383	3935.580631	23.519552
112.051354	3932.510768	23.524570
112.126042	3956.920589	23.529587
112.302573	3971.223860	23.534605
112.735631	3968.337635	23.539623
112.798963	3963.478960	23.544640
112.877404	3956.735436	23.549658
113.060939	3960.428485	23.554675
113.120639	3955.978696	23.559693
113.282271	3962.935328	23.564711
113.457045	3987.223931	23.569728
113.183420	3989.629085	23.574746
113.529686	3993.464944	23.579763
113.558352	3987.014289	23.584781
113.432108	3987.032793	23.589799
113.197434	4000.135088	23.594816
114.085755	4005.875165	23.599834
113.812277	4022.698215	23.604851
113.824967	4023.581988	23.609869
114.128327	4016.666229	23.614887
114.253548	4045.367624	23.619904
114.307888	4053.177100	23.624922
114.288348	4050.052246	23.629939
114.587603	4049.038590	23.634957
114.967541	4051.202292	23.639975
114.853758	4073.405545	23.644992
115.134843	4076.048991	23.650010
115.219897	4078.706324	23.655027
115.261410	4075.074504	23.660045
115.015131	4070.101987	23.665063
115.413220	4075.643159	23.670080
115.807408	4088.688865	23.675098
115.907939	4106.733336	23.680115
115.761249	4105.577604	23.685133
115.797001	4099.850569	23.690151
115.994622	4100.988054	23.695168
115.973397	4094.685369	23.700186
116.259768	4103.965657	23.705203
116.499599	4120.095699	23.710221
116.430019	4120.526514	23.715239
116.707588	4129.774412	23.720256
116.609278	4115.480131	23.725274
116.771403	4115.964790	23.730291
117.131294	4122.406822	23.735309
117.152265	4107.560924	23.740327
117.198678	4127.382949	23.745344
117.692209	4143.035641	23.750362
118.220158	4138.694659	23.755379
118.123274	4134.015562	23.760397
118.013218	4104.726837	23.765415
118.124968	4103.229569	23.770432
118.061056	4100.162826	23.775450
118.424248	4116.888259	23.780467
118.292498	4124.926561	23.785485
118.330834	4127.380982	23.790503
118.370754	4137.305585	23.795520
118.649817	4132.835642	23.800538
118.673854	4138.173670	23.805555
118.535208	4140.425041	23.810573
118.852792	4131.389454	23.815591
118.761735	4151.943315	23.820608
119.142226	4153.920711	23.825626
119.047923	4157.108899	23.830643
119.225360	4162.093620	23.835661
119.342236	4151.556462	23.840679
119.200181	4170.750201	23.845696
119.379914	4184.989751	23.850714
119.141726	4190.987299	23.855731
119.605339	4213.141805	23.860749
120.063821	4210.283622	23.865767
119.871186	4222.706286	23.870784
120.159092	4229.036235	23.875802
120.322536	4234.213458	23.880819
120.297838	4248.451803	23.885837
120.164458	4247.814362	23.890855
120.194051	4256.833216	23.895872
120.581950	4263.827011	23.900890
120.689456	4273.536978	23.905907
120.618537	4291.272571	23.910925
121.152587	4297.120905	23.915943
121.246888	4297.869548	23.920960
121.872632	4309.318819	23.925978
121.788695	4301.255833	23.930995
121.602224	4304.654962	23.936013
121.822683	4303.989763	23.941031
121.982946	4325.130315	23.946048
121.862334	4332.524325	23.951066
122.384778	4326.357318	23.956083
122.392583	4332.414674	23.961101
122.793914	4339.438962	23.966119
122.531827	4337.071101	23.971136
122.670252	4353.100023	23.976154
123.044986	4363.177335	23.981171
123.023662	4365.618421	23.986189
123.202564	4357.247392	23.991207
123.118998	4371.223512	23.996224
123.318534	4364.697220	24.001242
123.595213	4361.623758	24.006259
123.410890	4380.866081	24.011277
123.521572	4386.085540	24.016295
123.614433	4383.605869	24.021312
123.853337	4384.921606	24.026330
124.127720	4393.923716	24.031347
124.413129	4410.415451	24.036365
124.378019	4417.189427	24.041383
124.460674	4417.758491	24.046400
124.704161	4412.132853	24.051418
124.573868	4411.907521	24.056435
124.788890	4416.302215	24.061453
124.983892	4410.599543	24.066471
125.110988	4415.463521	24.071488
124.781877	4424.230697	24.076506
125.514051	4430.117217	24.081523
125.290728	4435.864354	24.086541
125.391645	4439.007350	24.091559
125.483616	4437.560566	24.096576
125.580004	4449.158041	24.101594
125.984439	4458.176891	24.106611
125.549155	4469.587803	24.111629
125.983926	4462.249713	24.116647
125.930538	4476.978867	24.121664
125.965380	4486.960047	24.126682
126.412320	4486.653904	24.131699
126.278608	4486.193292	24.136717
126.384273	4509.523587	24.141735
126.446720	4525.431373	24.146752
126.737859	4526.243967	24.151770
127.011047	4531.333466	24.156787
127.308718	4553.130414	24.161805
127.397090	4551.089287	24.166823
127.278793	4564.200779	24.171840
127.305759	4564.149082	24.176858
127.687948	4567.403514	24.181875
127.815197	4584.774782	24.186893
127.879385	4585.948526	24.191911
127.964239	4582.869707	24.196928
128.247271	4604.883335	24.201946
128.285289	4608.142279	24.206963
128.189701	4620.274792	24.211981
128.454659	4616.507099	24.216999
128.815748	4630.087511	24.222016
128.675029	4641.515235	24.227034
129.376862	4638.641178	24.232051
129.134408	4631.025508	24.237069
129.645914	4644.012529	24.242087
130.279673	4647.824279	24.247104
130.397137	4636.089356	24.252122
130.707054	4610.687695	24.257139
130.737093	4607.890784	24.262157
130.710839	4606.975764	24.267175
130.917408	4606.362853	24.272192
130.850361	4612.495683	24.277210
131.175719	4595.855973	24.282227
130.652313	4613.420222	24.287245
130.882614	4608.367210	24.292263
130.876789	4603.559530	24.297280
130.940216	4604.296359	24.302298
131.265751	4598.212574	24.307315
131.091836	4611.541974	24.312333
131.314405	4623.617195	24.317351
131.198410	4630.372342	24.322368
131.292612	4629.052348	24.327386
131.220255	4621.263289	24.332403
131.150205	4658.053055	24.337421
131.576272	4660.104883	24.342439
131.633953	4674.641054	24.347456
131.696266	4692.666533	24.352474
132.331147	4697.018707	24.357491
132.391391	4705.125592	24.362509
132.723037	4720.987128	24.367527
132.729413	4734.941624	24.372544
132.676719	4739.703115	24.377562
132.951291	4725.836863	24.382579
132.729495	4731.801985	24.387597
132.927001	4748.426723	24.392615
133.039460	4760.514338	24.397632
133.460126	4757.065796	24.402650
133.757631	4755.255465	24.407667
133.260662	4773.184060	24.412685
133.651361	4783.624000	24.417703
133.662270	4787.207962	24.422720
133.798632	4795.235381	24.427738
134.584650	4806.835327	24.432755
134.521606	4811.040230	24.437773
134.743960	4802.754313	24.442791
135.242790	4798.679405	24.447808
135.250021	4805.607985	24.452826
135.817263	4805.172502	24.457843
135.921650	4792.881696	24.462861
135.869728	4794.562088	24.467879
135.874466	4802.719931	24.472896
135.982520	4800.792066	24.477914
135.983952	4797.085984	24.482931
135.904058	4795.939637	24.487949
135.892028	4790.662016	24.492967
135.976702	4790.729141	24.497984
135.706243	4794.010350	24.503002
136.313224	4808.502740	24.508019
136.330519	4821.832223	24.513037
136.087631	4828.228860	24.518055
136.067603	4833.479516	24.523072
136.458417	4849.803499	24.528090
136.702537	4856.935503	24.533107
136.824900	4868.666413	24.538125
136.925692	4879.970934	24.543143
137.013605	4887.864267	24.548160
137.154913	4912.598073	24.553178
137.407207	4907.028288	24.558195
137.693844	4914.054465	24.563213
137.593056	4927.690193	24.568231
137.888123	4941.045542	24.573248
137.613567	4954.669449	24.578266
138.157883	4966.696893	24.583283
138.561900	4973.213100	24.588301
138.403089	4969.696464	24.593319
138.674035	4973.754878	24.598336
138.678006	4996.448699	24.603354
139.072162	4996.893867	24.608371
139.133702	4997.629058	24.613389
139.233969	5008.456937	24.618407
139.838634	5014.063539	24.623424
139.559318	5023.750084	24.628442
139.878529	5014.856650	24.633459
140.094685	5011.515869	24.638477
140.068699	5019.743081	24.643495
140.374435	5037.317669	24.648512
140.696095	5056.872930	24.653530
140.681642	5049.218201	24.658547
140.884823	5055.347897	24.663565
141.004511	5048.532908	24.668583
140.727040	5038.228833	24.673600
141.044449	5053.719793	24.678618
140.869973	5069.476314	24.683635
141.242636	5074.796040	24.688653
141.238174	5078.110924	24.693671
141.315861	5098.319608	24.698688
141.096478	5106.978472	24.703706
141.714910	5110.201861	24.708723
142.175227	5122.167705	24.713741
142.041998	5143.879966	24.718759
142.229687	5140.056011	24.723776
142.510754	5142.797688	24.728794
142.539610	5133.836795	24.733811
143.002738	5137.726868	24.738829
142.933780	5158.210675	24.743847
143.193434	5168.566216	24.748864
143.151050	5177.759717	24.753882
143.067715	5176.407193	24.758899
143.169557	5168.296526	24.763917
143.229846	5175.705535	24.768935
143.613232	5178.159021	24.773952
143.851116	5182.020567	24.778970
143.789078	5187.243634	24.783987
144.183359	5193.566638	24.789005
143.763810	5216.724503	24.794023
144.401999	5221.549566	24.799040
144.289105	5218.498177	24.804058
144.812627	5225.768852	24.809075
145.009665	5231.663385	24.814093
145.193176	5250.731418	24.819111
145.761597	5241.557674	24.824128
145.794831	5239.336176	24.829146
145.670714	5245.328271	24.834163
146.188317	5235.465600	24.839181
145.838079	5242.430995	24.844199
146.332644	5221.627918	24.849216
146.219960	5230.992141	24.854234
146.529958	5222.067431	24.859251
146.699970	5239.302819	24.864269
146.234371	5258.039478	24.869287
146.558288	5264.004802	24.874304
146.630159	5264.692624	24.879322
146.844946	5262.801405	24.884339
147.061630	5272.682560	24.889357
147.008528	5280.284786	24.894375
147.060774	5282.051967	24.899392
147.128668	5301.182478	24.904410
147.335057	5319.977097	24.909427
147.472289	5321.609359	24.914445
147.760412	5329.912804	24.919463
148.119669	5341.241496	24.924480
147.881870	5349.452692	24.929498
147.934526	5345.505311	24.934515
148.190646	5362.182836	24.939533
148.223320	5380.868812	24.944551
148.945218	5384.017283	24.949568
149.245841	5392.808916	24.954586
149.459492	5397.738437	24.959603
149.756624	5400.040048	24.964621
149.665142	5410.071433	24.969639
149.891735	5396.347968	24.974656
149.721158	5410.959945	24.979674
149.862806	5411.636244	24.984691
150.145738	5420.169758	24.989709
150.137039	5442.640699	24.994727
150.538278	5438.445516	24.999744
150.283133	5438.547530	25.004762
150.367640	5443.016450	25.009779
150.473026	5463.293479	25.014797
150.664765	5462.899157	25.019815
150.650454	5487.503659	25.024832
150.869800	5497.180945	25.029850
151.237031	5499.939162	25.034867
151.575299	5495.956758	25.039885
151.484047	5519.330546	25.044903
151.745552	5523.080385	25.049920
151.932147	5526.025955	25.054938
151.935847	5536.394893	25.059955
152.174811	5542.460199	25.064973
152.253928	5542.043533	25.069991
152.480036	5547.846362	25.075008
152.639413	5554.139814	25.080026
152.685576	5579.455434	25.085043
152.938774	5566.183789	25.090061
153.058076	5582.253358	25.095079
153.374392	5580.333119	25.100096
153.558623	5598.324927	25.105114
153.354689	5618.259902	25.110131
153.805424	5602.126835	25.115149
153.672524	5608.362680	25.120167
154.025286	5616.179544	25.125184
154.080217	5639.354529	25.130202
153.981643	5638.795936	25.135219
154.381070	5631.947073	25.140237
154.459835	5658.175677	25.145255
154.913240	5661.246110	25.150272
154.834850	5669.268117	25.155290
155.076756	5663.876974	25.160307
155.507538	5689.128434	25.165325
155.519564	5689.748593	25.170343
155.736302	5699.884378	25.175360
155.807101	5697.107708	25.180378
155.711456	5704.526982	25.185395
156.230233	5720.635823	25.190413
156.037602	5719.300523	25.195431
156.275638	5716.589931	25.200448
156.397362	5718.169278	25.205466
156.351870	5731.430764	25.210483
156.735157	5736.627290	25.215501
157.081539	5743.293918	25.220519
157.202725	5761.608976	25.225536
157.683873	5767.554027	25.230554
157.500285	5769.707527	25.235571
157.918335	5762.357817	25.240589
157.952691	5782.957673	25.245607
158.147397	5792.729386	25.250624
158.544242	5779.937447	25.255642
158.476093	5785.177079	25.260659
158.508057	5774.058281	25.265677
158.544430	5788.737218	25.270695
158.795026	5812.854690	25.275712
159.076621	5821.527643	25.280730
159.170757	5823.196611	25.285747
159.152024	5806.420713	25.290765
159.059194	5830.268920	25.295783
159.676614	5839.904666	25.300800
159.945340	5843.560856	25.305818
159.801538	5847.520677	25.310835
159.718970	5860.596242	25.315853
159.872830	5869.847896	25.320871
160.294452	5875.563416	25.325888
160.283745	5892.478932	25.330906
160.276688	5901.316964	25.335923
160.729555	5911.278416	25.340941
160.898176	5933.829047	25.345959
161.329825	5938.048201	25.350976
161.463547	5932.598451	25.355994
161.394841	5937.725608	25.361011
161.557587	5954.851154	25.366029
161.962839	5979.644232	25.371047
161.967534	5972.587170	25.376064
162.499861	5964.056875	25.381082
162.218269	5973.631761	25.386099
162.587284	5980.731832	25.391117
162.425874	5991.625678	25.396135
162.499736	5997.904299	25.401152
162.755511	6016.095037	25.406170
162.858399	6023.612389	25.411187
162.952723	6016.720843	25.416205
163.431957	6022.407210	25.421223
163.548380	6039.349131	25.426240
163.952198	6046.899464	25.431258
163.734102	6042.737938	25.436275
164.115925	6049.224008	25.441293
164.190679	6055.426113	25.446311
164.590547	6056.226341	25.451328
164.813625	6059.641263	25.456346
164.833250	6065.944623	25.461363
165.178280	6062.268100	25.466381
165.436813	6064.186357	25.471399
165.251789	6068.820877	25.476416
165.212624	6075.677355	25.481434
165.491038	6098.740883	25.486451
165.468898	6086.807038	25.491469
165.929176	6098.615739	25.496487
166.095119	6111.222030	25.501504
166.434059	6112.317417	25.506522
166.529473	6116.196041	25.511539
166.872546	6120.585025	25.516557
166.877177	6115.216395	25.521575
167.030395	6146.467467	25.526592
167.251684	6141.133909	25.531610
166.671394	6153.643808	25.536627
167.038716	6148.675952	25.541645
167.723932	6165.497253	25.546663
167.639149	6170.141229	25.551680
167.886878	6167.736889	25.556698
168.006336	6182.951384	25.561715
168.237024	6195.859700	25.566733
168.186541	6207.125989	25.571751
168.180953	6222.335193	25.576768
168.703562	6222.828484	25.581786
168.328042	6231.407050	25.586803
168.857398	6246.833459	25.591821
168.935492	6265.174338	25.596839
168.933807	6281.476858	25.601856
169.383691	6290.261662	25.606874
169.503927	6303.025293	25.611891
169.952751	6304.185231	25.616909
169.773821	6319.640534	25.621927
169.827218	6337.826493	25.626944
170.323682	6339.410141	25.631962
170.284766	6362.445369	25.636979
171.003591	6364.349041	25.641997
171.290311	6360.193802	25.647015
171.070464	6359.307122	25.652032
171.490373	6384.857619	25.657050
171.574341	6391.435573	25.662067
171.875497	6382.923561	25.667085
171.877656	6376.842514	25.672103
172.238348	6390.217793	25.677120
172.338595	6407.477805	25.682138
172.085191	6419.539338	25.687156
172.138173	6416.382734	25.692173
172.855141	6425.569241	25.697191
172.609766	6436.926174	25.702208
172.968068	6439.914820	25.707226
173.101806	6454.516075	25.712244
173.254752	6455.938340	25.717261
173.459904	6469.015699	25.722279
173.435474	6469.785248	25.727296
174.462998	6484.837398	25.732314
173.926624	6505.922341	25.737332
174.148527	6507.633277	25.742349
174.498154	6509.121495	25.747367
174.579648	6510.852481	25.752384
175.049995	6505.535142	25.757402
175.295120	6512.188114	25.762420
175.621625	6516.868195	25.767437
175.720297	6516.454968	25.772455
175.730396	6525.730762	25.777472
176.326906	6512.053102	25.782490
175.972953	6520.410107	25.787508
175.704552	6523.657466	25.792525
175.928476	6514.030358	25.797543
176.014695	6528.666310	25.802560
176.311627	6536.438520	25.807578
176.126438	6545.127569	25.812596
176.102767	6560.985888	25.817613
176.424493	6565.585654	25.822631
176.295264	6596.166818	25.827648
176.963699	6600.576999	25.832666
177.586632	6623.618240	25.837684
177.464908	6627.859708	25.842701
177.825285	6629.312296	25.847719
177.777144	6638.618256	25.852736
178.322226	6654.785144	25.857754
178.277063	6669.133420	25.862772
178.510032	6670.964619	25.867789
178.723419	6673.168423	25.872807
178.569016	6689.345385	25.877824
179.088680	6692.438944	25.882842
179.445578	6712.861502	25.887860
178.976076	6732.596830	25.892877
179.573113	6735.970590	25.897895
179.308605	6752.100440	25.902912
179.456047	6754.864876	25.907930
179.797369	6774.686021	25.912948
180.140257	6787.039161	25.917965
180.375257	6797.899569	25.922983
180.444314	6823.572543	25.928000
180.756499	6824.488899	25.933018
181.000353	6841.043619	25.938036
181.085147	6842.236969	25.943053
181.257846	6855.777594	25.948071
181.666602	6868.651529	25.953088
182.041372	6876.016471	25.958106
181.921568	6882.440067	25.963124
182.286291	6879.869013	25.968141
182.287706	6896.570959	25.973159
182.572599	6906.361543	25.978176
182.818544	6908.286711	25.983194
182.640900	6924.321263	25.988212
182.810950	6937.738747	25.993229
183.068362	6932.799833	25.998247
183.156167	6963.189908	26.003264
183.339648	6979.823268	26.008282
183.694678	6985.576190	26.013300
183.950963	6996.676582	26.018317
184.198557	7003.432529	26.023335
184.443984	7007.419691	26.028352
184.828954	7023.224346	26.033370
185.107587	7031.040779	26.038388
184.863655	7041.141708	26.043405
185.276909	7039.888906	26.048423
185.014169	7056.511014	26.053440
185.486410	7052.509239	26.058458
185.404432	7060.534122	26.063476
185.839017	7088.109799	26.068493
185.589017	7094.345494	26.073511
185.878620	7110.064395	26.078528
186.229792	7119.122729	26.083546
186.680329	7114.252662	26.088564
186.606989	7127.340353	26.093581
187.133111	7146.804584	26.098599
187.124363	7146.739090	26.103616
187.890240	7136.699149	26.108634
187.783451	7142.185830	26.113652
187.817615	7137.931926	26.118669
188.237959	7140.916759	26.123687
188.395903	7157.398583	26.128704
188.388400	7159.905159	26.133722
188.219901	7169.400649	26.138740
188.463732	7173.586590	26.143757
188.976928	7183.980727	26.148775
189.244616	7193.104091	26.153792
189.395069	7190.045429	26.158810
189.966533	7193.052559	26.163828
189.587238	7187.533559	26.168845
189.989514	7197.518368	26.173863
189.794636	7223.093834	26.178880
190.112851	7212.671791	26.183898
190.483334	7228.790935	26.188916
190.505836	7250.486276	26.193933
190.747307	7245.195482	26.198951
190.684108	7261.387100	26.203968
191.424361	7269.495978	26.208986
191.300397	7274.568903	26.214004
191.377668	7294.493400	26.219021
191.508626	7291.994772	26.224039
191.377457	7307.028084	26.229056
191.832601	7320.678387	26.234074
192.113820	7336.378422	26.239092
192.109012	7345.312192	26.244109
192.339008	7358.365708	26.249127
192.517608	7369.354758	26.254144
192.773010	7373.217499	26.259162
193.124906	7398.080702	26.264180
193.313631	7407.106185	26.269197
193.703394	7407.081961	26.274215
193.793949	7432.042742	26.279232
194.105272	7428.570740	26.284250
194.064117	7434.611391	26.289268
194.298015	7455.133209	26.294285
194.566202	7462.241949	26.299303
194.626177	7473.341245	26.304320
194.652633	7490.321645	26.309338
195.222370	7495.019328	26.314356
194.888636	7509.624761	26.319373
195.504342	7523.657482	26.324391
195.462818	7529.937664	26.329408
196.219580	7540.455618	26.334426
196.628542	7551.164150	26.339444
196.961724	7547.385281	26.344461
197.220480	7540.761257	26.349479
197.485157	7548.099024	26.354496
197.275854	7545.832999	26.359514
197.188647	7542.980509	26.364532
197.090501	7559.249879	26.369549
197.501284	7556.374180	26.374567
197.438219	7568.539033	26.379584
197.457863	7589.471328	26.384602
197.987381	7595.881657	26.389620
198.159748	7622.055535	26.394637
198.365345	7632.280259	26.399655
198.543350	7643.543689	26.404672
198.744005	7654.886084	26.409690
198.949507	7662.708613	26.414708
198.978456	7673.364235	26.419725
199.383909	7685.261165	26.424743
199.527384	7704.891698	26.429760
199.417485	7725.589600	26.434778
199.961266	7727.916181	26.439796
199.987888	7739.232257	26.444813
200.042732	7755.881388	26.449831
199.960258	7773.881944	26.454848
200.206434	7790.786195	26.459866
200.745800	7790.886904	26.464884
200.508222	7818.715111	26.469901
200.712455	7832.286020	26.474919
200.898585	7852.582321	26.479936
201.475516	7865.521440	26.484954
202.293147	7866.029848	26.489972
202.390331	7876.495541	26.494989
202.950413	7871.336991	26.500007
203.116627	7871.808103	26.505024
203.212606	7884.420285	26.510042
203.331652	7894.887104	26.515060
203.418042	7894.634973	26.520077
203.767765	7900.533245	26.525095
204.010073	7910.247214	26.530112
204.435611	7911.477289	26.535130
204.702089	7923.428866	26.540148
204.728708	7920.418879	26.545165
205.060004	7923.344539	26.550183
204.965089	7923.883213	26.555200
204.940266	7931.610034	26.560218
205.384802	7936.228508	26.565236
204.961389	7949.086445	26.570253
205.140273	7963.170464	26.575271
205.477736	7978.092329	26.580288
205.531380	7992.422330	26.585306
205.969939	8010.878174	26.590324
205.797014	8023.549072	26.595341
206.299473	8039.466084	26.600359
206.492003	8051.031432	26.605376
206.660944	8070.307713	26.610394
207.094638	8067.154040	26.615412
207.063299	8079.976447	26.620429
207.385534	8102.370902	26.625447
207.740368	8116.144800	26.630464
207.578313	8135.912988	26.635482
207.975076	8142.216303	26.640500
208.159765	8162.480947	26.645517
208.229702	8175.057493	26.650535
208.940446	8192.643918	26.655552
208.772984	8206.270258	26.660570
209.291076	8207.432293	26.665588
209.411093	8230.769282	26.670605
209.522575	8240.600374	26.675623
209.951757	8258.628002	26.680640
210.073664	8270.183124	26.685658
210.754750	8260.413264	26.690676
210.509320	8277.823012	26.695693
210.729665	8293.436388	26.700711
211.076613	8291.777783	26.705728
210.825600	8317.326480	26.710746
211.191251	8323.640521	26.715764
211.098878	8338.158790	26.720781
211.618297	8352.293226	26.725799
211.669231	8367.228929	26.730816
212.053898	8398.244579	26.735834
211.965822	8404.022399	26.740852
212.082334	8414.835760	26.745869
212.541180	8424.558378	26.750887
213.129853	8440.156728	26.755904
213.089403	8464.551613	26.760922
213.495288	8464.379801	26.765940
213.728785	8478.867201	26.770957
213.926563	8488.865351	26.775975
214.521855	8484.567212	26.780992
214.479278	8489.887792	26.786010
214.669899	8506.590895	26.791028
214.853344	8507.410476	26.796045
214.911853	8514.055746	26.801063
215.525925	8511.886691	26.806080
215.379556	8530.175917	26.811098
215.848689	8520.503930	26.816116
216.114628	8531.709355	26.821133
215.869685	8528.620458	26.826151
216.470470	8546.269553	26.831168
216.523298	8560.250481	26.836186
216.619710	8566.165650	26.841204
216.915286	8585.980876	26.846221
216.732948	8591.237938	26.851239
216.940500	8596.306922	26.856256
217.129571	8631.288936	26.861274
217.344828	8645.708612	26.866292
217.853006	8651.421878	26.871309
217.442202	8664.557141	26.876327
217.926151	8686.597247	26.881344
218.080267	8705.739696	26.886362
219.108043	8700.773781	26.891380
219.633597	8714.251400	26.896397
220.021343	8733.306447	26.901415
220.139517	8740.018359	26.906432
220.264122	8742.719967	26.911450
220.516791	8737.092069	26.916468
220.800244	8748.847699	26.921485
220.521788	8744.603269	26.926503
221.022066	8742.234800	26.931520
220.864147	8760.177260	26.936538
221.198669	8766.547822	26.941556
221.362251	8771.991182	26.946573
221.405612	8797.769275	26.951591
221.470855	8805.363488	26.956608
221.301146	8823.650606	26.961626
221.781631	8836.939645	26.966644
222.063329	8867.285585	26.971661
221.994157	8876.586881	26.976679
222.558255	8898.573081	26.981696
222.555250	8919.428166	26.986714
222.574250	8931.787664	26.991732
223.198940	8955.304634	26.996749
223.276779	8967.068403	27.001767
223.860576	8998.078320	27.006784
223.925254	9008.123206	27.011802
224.163747	9020.797816	27.016820
224.462433	9028.596962	27.021837
224.682965	9049.054525	27.026855
225.028886	9065.241828	27.031872
224.968138	9079.613765	27.036890
225.345700	9095.962862	27.041908
225.434796	9110.103695	27.046925
225.254332	9132.257344	27.051943
226.043239	9147.479877	27.056960
226.114243	9174.701000	27.061978
226.409832	9166.809912	27.066996
227.015960	9186.937705	27.072013
227.178904	9195.267422	27.077031
227.675054	9219.571659	27.082048
227.428933	9226.522770	27.087066
227.965723	9221.743369	27.092084
228.118031	9232.174068	27.097101
228.145083	9248.263003	27.102119
228.727301	9254.933911	27.107136
229.002226	9276.447745	27.112154
229.060041	9273.959317	27.117172
229.561386	9279.250949	27.122189
229.506644	9291.212518	27.127207
229.625995	9293.602373	27.132224
229.823137	9315.744303	27.137242
229.374642	9317.134652	27.142260
230.277193	9330.945936	27.147277
229.729774	9342.691192	27.152295
230.131234	9366.170821	27.157312
230.433582	9389.145401	27.162330
230.784329	9414.604312	27.167348
231.061626	9413.416334	27.172365
231.314296	9441.260904	27.177383
231.495813	9448.853544	27.182400
231.844542	9471.638620	27.187418
232.003467	9481.606005	27.192436
232.093647	9503.987214	27.197453
232.252149	9533.390623	27.202471
232.745851	9533.075900	27.207488
232.977726	9553.568472	27.212506
233.577864	9565.607163	27.217524
233.676046	9566.945811	27.222541
233.669737	9591.533709	27.227559
233.960577	9604.556969	27.232576
234.253998	9623.864983	27.237594
234.694547	9634.328670	27.242612
234.904385	9647.756843	27.247629
235.338629	9662.678484	27.252647
235.774652	9657.386260	27.257664
235.646598	9682.622222	27.262682
235.904207	9696.623879	27.267700
236.162034	9702.649078	27.272717
236.053357	9733.569243	27.277735
236.670782	9739.503537	27.282752
236.996653	9757.438082	27.287770
236.929285	9773.871627	27.292788
237.064904	9776.150949	27.297805
237.069841	9798.036210	27.302823
237.744194	9807.238838	27.307840
237.965127	9827.754838	27.312858
237.790562	9840.313230	27.317876
238.147963	9862.724051	27.322893
238.375781	9879.818676	27.327911
238.630017	9897.663598	27.332928
238.952822	9918.019517	27.337946
239.270805	9937.081232	27.342964
239.621446	9944.891151	27.347981
239.899927	9958.817907	27.352999
240.326892	9965.992131	27.358016
240.822623	9981.118964	27.363034
240.573827	9995.596839	27.368052
240.934266	9991.751454	27.373069
241.043036	10018.470717	27.378087
241.352255	10016.092672	27.383104
241.584848	10043.479998	27.388122
241.694057	10059.976041	27.393140
242.508692	10074.251510	27.398157
242.332430	10080.772373	27.403175
242.583259	10082.761724	27.408192
243.184662	10102.814261	27.413210
243.101874	10108.201892	27.418228
243.538923	10118.907525	27.423245
243.521984	10144.628435	27.428263
243.974432	10154.624946	27.433280
243.678805	10164.548120	27.438298
243.883284	10184.839641	27.443316
243.988190	10202.124283	27.448333
244.365784	10228.049552	27.453351
244.667840	10240.676033	27.458368
245.111309	10252.175530	27.463386
245.345384	10256.617557	27.468404
245.875850	10258.961693	27.473421
246.049260	10275.676585	27.478439
246.193981	10282.337497	27.483456
246.379100	10302.020286	27.488474
246.496951	10305.746561	27.493492
247.072346	10319.987730	27.498509
246.730009	10339.507205	27.503527
247.219916	10351.062120	27.508544
247.341608	10368.402462	27.513562
247.559107	10375.665834	27.518580
248.086057	10390.355422	27.523597
248.143785	10415.089982	27.528615
248.587310	10430.341666	27.533632
248.949438	10444.035243	27.538650
248.763209	10461.504545	27.543668
249.109085	10473.062076	27.548685
249.394308	10487.311160	27.553703
249.588291	10506.313690	27.558720
250.044095	10529.409507	27.563738
250.307136	10545.411919	27.568756
250.733951	10545.847151	27.573773
251.047089	10558.587066	27.578791
251.302824	10576.740513	27.583808
251.658602	10590.187120	27.588826
251.582640	10602.430467	27.593844
252.032368	10612.120488	27.598861
252.149282	10635.115682	27.603879
252.579224	10640.060350	27.608896
252.653731	10643.515784	27.613914
252.454910	10661.898828	27.618932
252.835232	10679.262162	27.623949
252.920868	10711.734735	27.628967
253.470799	10717.756963	27.633984
253.992303	10731.172370	27.639002
254.121813	10748.145519	27.644020
254.405108	10751.949338	27.649037
255.045650	10776.807956	27.654055
254.610820	10790.522421	27.659072
255.182202	10815.030149	27.664090
255.186036	10830.304441	27.669108
256.153747	10829.084226	27.674125
256.271657	10857.583748	27.679143
256.691388	10862.085867	27.684160
256.858674	10872.486017	27.689178
256.920343	10896.989062	27.694196
257.162611	10894.779506	27.699213
257.232688	10905.907099	27.704231
257.552810	10923.695016	27.709248
258.041555	10935.787026	27.714266
257.819762	10961.884199	27.719284
258.314743	10966.121038	27.724301
258.624125	10984.574895	27.729319
258.529068	10995.157903	27.734336
258.749881	11025.458923	27.739354
259.164435	11039.089204	27.744372
259.501379	11050.831395	27.749389
260.256308	11061.715179	27.754407
260.259600	11083.229057	27.759424
260.388469	11093.535648	27.764442
260.581915	11105.087309	27.769460
260.965785	11118.698306	27.774477
261.089832	11136.312452	27.779495
261.274938	11149.350504	27.784512
261.729355	11161.218322	27.789530
261.491179	11189.828469	27.794548
261.880560	11193.499063	27.799565
262.326533	11226.764748	27.804583
262.402591	11233.932134	27.809600
262.663355	11242.263303	27.814618
262.695216	11270.832921	27.819636
262.938250	11286.273742	27.824653
263.314444	11308.974183	27.829671
263.249402	11329.834781	27.834688
263.708531	11351.777900	27.839706
264.134962	11378.019962	27.844724
264.374383	11392.247482	27.849741
264.753206	11410.651755	27.854759
265.056095	11426.216748	27.859776
265.673732	11430.402724	27.864794
265.698327	11453.414343	27.869812
266.413451	11470.167821	27.874829
266.418685	11485.553585	27.879847
266.713005	11493.076567	27.884864
266.871392	11515.383931	27.889882
266.890110	11529.137535	27.894900
267.179068	11542.238318	27.899917
267.741665	11554.954357	27.904935
267.476050	11575.100778	27.909952
268.349802	11580.296996	27.914970
268.798572	11592.148735	27.919988
269.127321	11597.538202	27.925005
269.335281	11621.528953	27.930023
269.468212	11634.933686	27.935040
269.957354	11634.369952	27.940058
270.023738	11658.749694	27.945076
270.440298	11658.869956	27.950093
270.641008	11692.890887	27.955111
271.178289	11680.255381	27.960128
271.790603	11682.664994	27.965146
272.204558	11697.891262	27.970164
272.174848	11702.494659	27.975181
272.559407	11715.103948	27.980199
272.474726	11716.327243	27.985216
272.733677	11716.278165	27.990234
272.906933	11745.062398	27.995252
272.951094	11756.273644	28.000269
273.285307	11769.330896	28.005287
272.887685	11792.556137	28.010304
273.281824	11804.035754	28.015322
273.628503	11829.432218	28.020340
273.918761	11847.909924	28.025357
274.263441	11878.886949	28.030375
274.412680	11894.035023	28.035392
274.676469	11914.065256	28.040410
275.063275	11934.111429	28.045428
275.384706	11953.159220	28.050445
276.083955	11977.779171	28.055463
275.871187	12005.462444	28.060480
276.594311	12016.535701	28.065498
276.616665	12025.739404	28.070516
276.742392	12052.935891	28.075533
277.382230	12070.394943	28.080551
277.277836	12087.462511	28.085568
277.984884	12104.101389	28.090586
277.848188	12112.116574	28.095604
278.413740	12126.146691	28.100621
278.428907	12139.549241	28.105639
278.511522	12177.262028	28.110656
279.213836	12188.655555	28.115674
279.068202	12210.530375	28.120692
279.503074	12228.506408	28.125709
280.068398	12245.758940	28.130727
279.858649	12273.960575	28.135744
280.422697	12275.941001	28.140762
280.917866	12307.084646	28.145780
281.626583	12309.110507	28.150797
281.826008	12310.049768	28.155815
282.399357	12327.583900	28.160832
282.307997	12332.864968	28.165850
282.686572	12338.643529	28.170868
282.502385	12346.273540	28.175885
282.677505	12359.504095	28.180903
282.919190	12392.014943	28.185920
283.308604	12397.624710	28.190938
283.736158	12427.662588	28.195956
283.363668	12444.957607	28.200973
283.912697	12457.285043	28.205991
284.309294	12471.134594	28.211008
284.520269	12485.490687	28.216026
284.931737	12514.414206	28.221044
284.843351	12531.120336	28.226061
285.292866	12556.889371	28.231079
285.365204	12570.028355	28.236096
285.728604	12597.535516	28.241114
286.125970	12635.083922	28.246132
286.376425	12642.842384	28.251149
287.121251	12648.191830	28.256167
287.619164	12669.154969	28.261184
288.031946	12685.264774	28.266202
288.182406	12701.451023	28.271220
288.613774	12720.633618	28.276237
288.605055	12717.010882	28.281255
288.781569	12747.577730	28.286272
288.994212	12763.240079	28.291290
289.488276	12788.130742	28.296308
289.288435	12807.039542	28.301325
289.944882	12818.210250	28.306343
289.869150	12848.243816	28.311360
290.110647	12873.726272	28.316378
290.228781	12902.248284	28.321396
290.577551	12928.995764	28.326413
290.770048	12944.273982	28.331431
290.883637	12975.540260	28.336448
291.550791	13003.640840	28.341466
291.438014	13039.771191	28.346484
292.147596	13068.919060	28.351501
292.565060	13096.437049	28.356519
293.072564	13109.586519	28.361536
293.358362	13130.415117	28.366554
293.902756	13149.499185	28.371572
294.129340	13167.948741	28.376589
294.664158	13183.698516	28.381607
294.852655	13196.122325	28.386624
295.715490	13202.467265	28.391642
295.780405	13222.717919	28.396660
295.837218	13227.837706	28.401677
296.484971	13233.739154	28.406695
296.679222	13250.831096	28.411712
297.030218	13261.162258	28.416730
297.259138	13279.266459	28.421748
297.073499	13297.038917	28.426765
297.461166	13304.392113	28.431783
297.480779	13309.787531	28.436800
297.722563	13334.216463	28.441818
298.017876	13356.257139	28.446836
298.045427	13373.846337	28.451853
298.661530	13398.713053	28.456871
298.996985	13421.443690	28.461888
299.623752	13441.313425	28.466906
300.302009	13446.910511	28.471924
300.569035	13478.672427	28.476941
301.121176	13486.055263	28.481959
300.807677	13496.772120	28.486976
300.901951	13488.477263	28.491994
301.869549	13501.543165	28.497012
301.461599	13517.688539	28.502029
301.819371	13529.878209	28.507047
302.048074	13548.959750	28.512064
302.198855	13570.417908	28.517082
302.703440	13578.156898	28.522100
302.421319	13614.626941	28.527117
303.130646	13629.256280	28.532135
303.479846	13636.912237	28.537152
303.668567	13659.528777	28.542170
304.181695	13667.077300	28.547188
304.246268	13704.744625	28.552205
304.506218	13708.039289	28.557223
304.866669	13730.521977	28.562240
305.073611	13750.712007	28.567258
305.461460	13771.841314	28.572276
305.874737	13795.558698	28.577293
306.111473	13812.039092	28.582311
306.329405	13838.526041	28.587328
306.829661	13869.734893	28.592346
306.776521	13895.488250	28.597364
306.929307	13928.257975	28.602381
307.533061	13940.974623	28.607399
307.940904	13969.745336	28.612416
308.295394	13986.293126	28.617434
308.645258	14004.751635	28.622452
308.882547	14034.105339	28.627469
309.297493	14053.394661	28.632487
309.722288	14068.599318	28.637504
310.073643	14095.959735	28.642522
310.579354	14104.578126	28.647540
310.511894	14137.367323	28.652557
311.324842	14141.021417	28.657575
311.290086	14162.184804	28.662592
311.234716	14190.997764	28.667610
311.931132	14207.082717	28.672628
312.017604	14237.709798	28.677645
312.479884	14255.729262	28.682663
312.411300	14278.746896	28.687680
312.952675	14301.547180	28.692698
313.459799	14308.357907	28.697716
313.668473	14346.976811	28.702733
314.247696	14375.225100	28.707751
314.488722	14395.744391	28.712768
314.466461	14418.054873	28.717786
314.853694	14436.646378	28.722804
314.925785	14470.899264	28.727821
315.539780	14485.992686	28.732839
315.750005	14522.265230	28.737856
315.768364	14551.238420	28.742874
316.539100	14570.444364	28.747892
316.574225	14596.961172	28.752909
317.223338	14617.501577	28.757927
317.024137	14643.360617	28.762944
317.484917	14668.774997	28.767962
317.543864	14701.908484	28.772980
317.910086	14737.367773	28.777997
318.929627	14740.095904	28.783015
319.395416	14761.435829	28.788032
319.869515	14785.168249	28.793050
320.079902	14790.606711	28.798068
319.888115	14828.493915	28.803085
320.522895	14847.503594	28.808103
320.734203	14867.803030	28.813120
320.745663	14896.393443	28.818138
321.236328	14908.100445	28.823156
321.082706	14940.751048	28.828173
321.868195	14961.866643	28.833191
321.988753	14977.831590	28.838208
322.344029	15008.217142	28.843226
323.050698	15028.603571	28.848244
322.942103	15050.721153	28.853261
323.092605	15079.646659	28.858279
323.555739	15090.367062	28.863296
323.861339	15122.076960	28.868314
324.010075	15146.667400	28.873332
324.057542	15183.176329	28.878349
324.716090	15209.547014	28.883367
325.258895	15237.894225	28.888384
325.367980	15264.554344	28.893402
325.717395	15292.995062	28.898420
325.867828	15319.798159	28.903437
326.469919	15350.761360	28.908455
326.739051	15375.259759	28.913472
326.848041	15407.803294	28.918490
327.867170	15423.990591	28.923508
327.895636	15441.479430	28.928525
328.437989	15461.283637	28.933543
328.836417	15487.191849	28.938560
328.535002	15520.957040	28.943578
328.941229	15540.785407	28.948596
329.300078	15576.619676	28.953613
329.693698	15600.571460	28.958631
329.886923	15636.814616	28.963648
330.311630	15678.056563	28.968666
330.573284	15697.001217	28.973684
330.659027	15737.996716	28.978701
331.149612	15756.564775	28.983719
331.507657	15787.887479	28.988736
331.794760	15827.883833	28.993754
332.318771	15852.870388	28.998772
332.847445	15882.905834	29.003789
332.733415	15908.149177	29.008807
333.539878	15928.175095	29.013824
334.143837	15958.264436	29.018842
335.084363	15971.533823	29.023860
335.557762	16003.729926	29.028877
335.902852	16001.781664	29.033895
336.001579	16015.458079	29.038912
336.124139	16037.970645	29.043930
336.777721	16065.248189	29.048948
336.640655	16084.908495	29.053965
337.038286	16108.868242	29.058983
337.330974	16114.599307	29.064000
337.428406	16143.310083	29.069018
338.342323	16163.134140	29.074036
338.708970	16183.360690	29.079053
339.173535	16198.994187	29.084071
339.396245	16208.752667	29.089088
339.598237	16233.324909	29.094106
340.359507	16242.502705	29.099124
340.740064	16243.254673	29.104141
340.732674	16268.534540	29.109159
341.256145	16270.793269	29.114176
341.402759	16297.987888	29.119194
341.582100	16301.737702	29.124212
341.948096	16342.407873	29.129229
341.827609	16358.937247	29.134247
341.938044	16359.662921	29.139264
342.514750	16399.534024	29.144282
343.010680	16426.634901	29.149300
342.799062	16449.267855	29.154317
342.923760	16482.256963	29.159335
343.385409	16516.033685	29.164352
343.854989	16532.697442	29.169370
344.122127	16554.526446	29.174388
344.315590	16594.901068	29.179405
344.272205	16636.145525	29.184423
344.935082	16653.217207	29.189440
345.180944	16697.402342	29.194458
346.043968	16728.416462	29.199476
346.008320	16763.357062	29.204493
346.453224	16777.891076	29.209511
347.290476	16798.871261	29.214528
347.301955	16831.901838	29.219546
347.772129	16861.390794	29.224564
348.387311	16889.222973	29.229581
348.757397	16906.188826	29.234599
349.208156	16924.613482	29.239616
348.972357	16954.862295	29.244634
349.395942	16982.262897	29.249652
350.253564	16996.949586	29.254669
350.601254	17037.016109	29.259687
351.194062	17042.020177	29.264704
350.871862	17079.483340	29.269722
351.607542	17109.661791	29.274740
351.734389	17128.887283	29.279757
352.003859	17165.055019	29.284775
352.403022	17182.608991	29.289792
352.669759	17214.631980	29.294810
353.046357	17244.061425	29.299828
353.413075	17268.696268	29.304845
353.567191	17309.410138	29.309863
354.265599	17332.321114	29.314880
354.604729	17352.534737	29.319898
355.545745	17381.819175	29.324916
355.711297	17398.833511	29.329933
356.034044	17426.339778	29.334951
356.189456	17440.865460	29.339968
356.461526	17473.427128	29.344986
356.880075	17505.937867	29.350004
357.170024	17526.714649	29.355021
357.032081	17550.867428	29.360039
357.726115	17583.616527	29.365056
357.776700	17621.161192	29.370074
358.290557	17648.592125	29.375092
358.922981	17666.303530	29.380109
358.930133	17712.589349	29.385127
359.532050	17743.371108	29.390144
359.761341	17775.401373	29.395162
360.082108	17815.166872	29.400180
360.454195	17839.344577	29.405197
360.850560	17881.892394	29.410215
361.264379	17908.517495	29.415232
361.241391	17944.998483	29.420250
361.864674	17979.765027	29.425268
362.602162	18010.789698	29.430285
362.531496	18046.820100	29.435303
363.214915	18059.663943	29.440320
363.750297	18094.040155	29.445338
364.750590	18109.473485	29.450356
365.032556	18138.860262	29.455373
365.085381	18151.655451	29.460391
365.782313	18165.083512	29.465408
365.582397	18197.682018	29.470426
365.845388	18223.938479	29.475444
366.263088	18239.602155	29.480461
366.562023	18280.902932	29.485479
367.166191	18308.956858	29.490496
367.422499	18332.908513	29.495514
367.593978	18360.411376	29.500532
367.976136	18391.355172	29.505549
368.199278	18412.317495	29.510567
368.436013	18438.509278	29.515584
368.641303	18462.289852	29.520602
368.978349	18500.373991	29.525620
369.593054	18541.170860	29.530637
369.601165	18566.240461	29.535655
370.233099	18588.907232	29.540672
370.351221	18622.333607	29.545690
370.806676	18666.257672	29.550708
371.224383	18683.206455	29.555725
371.888549	18719.219388	29.560743
372.634841	18737.294602	29.565760
373.329849	18763.253563	29.570778
373.480181	18780.082678	29.575796
373.876891	18812.913283	29.580813
373.962542	18839.745422	29.585831
374.140657	18861.029438	29.590848
374.808479	18893.753941	29.595866
375.059301	18915.834672	29.600884
375.733179	18938.433517	29.605901
375.802258	18962.954541	29.610919
376.089504	18992.663533	29.615936
376.570946	19029.123478	29.620954
376.643268	19065.950592	29.625972
377.594735	19079.599025	29.630989
377.815998	19118.734639	29.636007
378.029511	19142.828524	29.641024
378.217213	19163.305831	29.646042
378.816007	19196.061250	29.651060
379.263880	19214.206776	29.656077
379.587266	19237.633190	29.661095
380.156430	19284.043364	29.666112
380.474159	19307.114553	29.671130
380.960779	19340.851947	29.676148
380.954731	19358.681676	29.681165
381.680597	19395.972206	29.686183
382.187992	19422.789214	29.691200
382.442356	19464.073501	29.696218
382.350261	19495.575344	29.701236
383.094688	19528.668354	29.706253
383.385718	19552.344897	29.711271
383.594777	19582.881276	29.716288
383.831219	19620.713465	29.721306
384.194917	19660.238263	29.726324
384.429564	19699.516484	29.731341
384.548779	19737.363574	29.736359
385.306650	19760.624368	29.741376
385.884170	19789.623165	29.746394
386.612036	19844.325826	29.751412
386.995644	19871.868665	29.756429
387.160060	19906.599977	29.761447
387.952727	19934.236141	29.766464
388.183880	19960.960924	29.771482
388.560861	19988.665846	29.776500
389.100845	20017.478918	29.781517
389.411961	20056.975509	29.786535
389.317640	20086.424739	29.791552
389.832159	20120.980431	29.796570
390.203228	20151.591982	29.801588
390.661262	20176.074186	29.806605
391.374573	20213.642927	29.811623
391.551478	20237.112287	29.816640
392.241865	20263.820023	29.821658
392.679302	20300.706210	29.826676
393.139635	20319.164600	29.831693
393.364631	20348.214723	29.836711
393.785399	20368.907246	29.841728
394.460887	20388.548780	29.846746
394.254966	20421.269286	29.851764
394.386856	20440.562419	29.856781
394.682290	20479.282246	29.861799
395.066977	20505.539550	29.866816
395.577966	20533.994139	29.871834
395.742374	20580.232008	29.876852
396.358424	20613.411443	29.881869
396.558699	20644.211336	29.886887
396.474133	20686.298739	29.891904
396.625080	20717.537298	29.896922
397.057094	20765.848710	29.901940
397.649027	20820.908093	29.906957
398.046167	20871.997072	29.911975
398.490858	20916.731297	29.916992
398.881437	20946.514987	29.922010
400.100609	20972.496444	29.927028
400.674076	21012.185280	29.932045
400.802050	21046.986466	29.937063
401.236996	21089.916062	29.942080
401.809087	21118.938565	29.947098
402.455932	21147.909356	29.952116
402.654292	21176.202273	29.957133
402.924042	21207.940803	29.962151
403.133053	21241.781504	29.967168
403.916681	21279.088780	29.972186
404.212584	21316.807781	29.977204
404.740545	21340.640062	29.982221
405.159346	21366.271920	29.987239
405.571935	21408.972697	29.992256
405.965676	21435.904735	29.997274
406.122736	21469.057634	30.002292
406.791461	21503.809856	30.007309
407.210779	21528.986249	30.012327
407.474842	21562.977738	30.017344
408.050158	21591.932735	30.022362
408.310249	21630.030430	30.027380
409.254503	21652.979296	30.032397
409.578185	21686.256453	30.037415
409.751895	21717.787937	30.042432
410.108413	21751.066105	30.047450
410.285275	21796.319898	30.052468
410.796523	21831.474043	30.057485
410.960873	21866.983544	30.062503
411.517548	21901.559601	30.067520
412.248505	21922.742008	30.072538
412.499263	21973.396576	30.077556
412.899182	22004.069813	30.082573
413.497358	22038.603035	30.087591
413.492381	22063.101422	30.092608
414.638066	22084.830411	30.097626
414.631015	22112.791482	30.102644
415.607116	22130.599091	30.107661
416.130272	22160.812378	30.112679
415.909156	22189.728115	30.117696
416.719866	22229.790570	30.122714
416.764584	22262.553665	30.127732
417.177389	22285.838722	30.132749
417.383181	22317.569418	30.137767
417.498656	22353.154237	30.142784
417.943780	22385.200272	30.147802
418.283316	22436.264110	30.152820
419.013053	22459.979513	30.157837
419.231845	22515.072983	30.162855
419.194522	22562.749711	30.167872
419.703272	22602.371012	30.172890
420.096106	22644.445943	30.177908
420.838182	22682.647721	30.182925
421.387876	22715.096508	30.187943
421.426689	22756.490733	30.192960
422.497155	22790.214323	30.197978
422.633451	22826.151455	30.202996
422.813929	22855.107631	30.208013
422.769014	22905.993584	30.213031
423.427776	22940.482385	30.218048
424.018037	22978.298391	30.223066
424.167184	23023.631008	30.228084
424.720326	23058.049200	30.233101
425.467093	23105.602669	30.238119
425.727902	23155.257907	30.243136
426.596281	23180.102434	30.248154
427.028407	23219.602243	30.253172
427.235445	23253.294369	30.258189
427.765257	23301.071858	30.263207
427.642159	23339.331316	30.268224
428.111744	23375.821607	30.273242
428.540853	23415.913653	30.278260
428.874088	23458.541282	30.283277
429.894260	23492.474835	30.288295
430.340750	23527.608528	30.293312
431.188399	23561.733124	30.298330
431.317466	23610.232040	30.303348
431.534356	23648.781348	30.308365
432.317924	23684.641766	30.313383
432.403750	23718.760071	30.318400
433.303097	23759.095340	30.323418
433.823965	23808.495094	30.328436
434.149417	23834.865145	30.333453
434.408301	23865.133023	30.338471
434.877054	23904.350864	30.343488
435.425475	23929.873760	30.348506
435.856722	23974.093253	30.353524
436.321277	24012.980911	30.358541
436.590770	24036.908588	30.363559
437.234807	24083.269211	30.368576
437.476253	24112.217466	30.373594
437.953762	24150.463113	30.378612
438.618002	24195.089359	30.383629
438.993294	24215.972314	30.388647
439.149679	24257.699263	30.393664
440.086640	24292.296245	30.398682
440.279225	24333.243175	30.403700
440.337375	24371.186457	30.408717
441.078509	24400.435835	30.413735
441.290144	24448.245463	30.418752
442.039073	24477.014325	30.423770
442.533915	24521.076515	30.428788
442.848892	24563.186421	30.433805
443.252913	24595.260780	30.438823
443.546112	24641.182592	30.443840
444.075122	24673.036190	30.448858
444.413579	24719.447450	30.453876
444.662513	24758.279397	30.458893
445.440404	24807.146039	30.463911
445.666397	24851.712366	30.468928
445.756653	24891.094350	30.473946
446.096364	24936.727013	30.478964
446.101408	24975.233901	30.483981
446.963314	25029.513397	30.488999
447.672179	25087.289114	30.494016
448.047405	25127.603830	30.499034
448.451651	25170.362793	30.504052
448.963390	25205.602718	30.509069
449.941439	25254.592121	30.514087
450.199662	25302.331795	30.519104
450.791259	25335.407873	30.524122
451.343973	25368.704901	30.529140
451.602909	25405.638045	30.534157
452.366806	25434.451787	30.539175
452.591522	25478.736114	30.544192
453.315029	25513.567962	30.549210
453.760199	25528.793951	30.554228
453.787270	25567.743235	30.559245
454.499951	25600.164316	30.564263
454.928860	25640.671650	30.569280
455.306756	25670.429494	30.574298
455.303242	25704.041405	30.579316
455.743774	25744.326291	30.584333
456.040406	25787.637590	30.589351
456.587113	25839.476966	30.594368
456.994764	25879.344971	30.599386
457.449689	25934.356905	30.604404
457.816367	25980.483075	30.609421
458.418417	26025.996466	30.614439
458.545496	26085.365070	30.619456
458.993657	26132.768174	30.624474
459.494912	26188.252679	30.629492
459.915674	26240.965657	30.634509
460.564903	26285.509968	30.639527
461.143978	26345.435618	30.644544
461.469533	26387.368494	30.649562
462.244222	26433.718661	30.654580
462.271967	26478.350360	30.659597
463.189756	26534.867952	30.664615
463.366884	26587.158589	30.669632
464.116117	26635.566817	30.674650
464.544897	26683.488762	30.679668
465.080364	26733.743033	30.684685
465.669089	26776.838261	30.689703
466.468826	26817.012716	30.694720
466.570929	26849.792506	30.699738
466.993830	26908.228780	30.704756
467.466749	26953.409544	30.709773
468.765418	26974.750531	30.714791
469.281279	27023.627368	30.719808
469.537277	27049.427185	30.724826
470.209095	27091.232039	30.729844
470.647441	27122.613130	30.734861
470.963749	27171.409798	30.739879
471.182862	27205.565091	30.744896
471.793177	27250.919504	30.749914
472.346608	27290.104326	30.754932
472.722578	27335.128626	30.759949
473.671202	27353.474620	30.764967
474.414909	27395.814022	30.769984
474.545983	27426.022578	30.775002
475.258159	27459.831978	30.780020
475.486266	27495.364766	30.785037
475.680001	27518.210574	30.790055
476.060004	27554.106367	30.795072
476.381394	27602.878184	30.800090
476.739146	27638.352001	30.805108
476.996680	27686.569987	30.810125
477.610920	27729.360578	30.815143
477.957006	27777.570499	30.820160
478.441484	27831.930686	30.825178
479.100657	27873.171753	30.830196
479.369914	27924.211583	30.835213
480.106790	27955.087504	30.840231
480.565084	28015.471067	30.845248
480.523299	28055.386815	30.850266
481.298163	28106.403602	30.855284
481.947746	28145.123412	30.860301
482.575290	28176.402622	30.865319
483.113079	28220.841027	30.870336
483.433564	28265.583563	30.875354
483.991497	28297.691478	30.880372
484.131717	28337.347542	30.885389
484.938506	28380.221501	30.890407
484.966377	28425.470173	30.895424
485.106629	28479.756770	30.900442
485.544044	28523.300901	30.905460
485.738028	28571.793670	30.910477
486.394574	28629.506358	30.915495
486.679453	28690.081797	30.920512
487.187277	28733.520192	30.925530
487.747665	28793.835982	30.930548
488.228692	28865.117515	30.935565
488.625342	28914.445255	30.940583
489.375800	28971.074190	30.945600
489.785321	29021.324382	30.950618
490.600218	29077.643341	30.955636
491.007840	29147.528080	30.960653
492.051518	29170.547982	30.965671
492.736522	29218.687010	30.970688
492.927131	29270.393636	30.975706
493.628032	29315.829991	30.980724
494.059428	29367.415116	30.985741
494.944524	29402.439513	30.990759
496.025358	29435.889049	30.995776
497.289637	29454.645725	31.000794
497.824043	29477.803785	31.005812
498.017747	29496.753110	31.010829
498.555572	29525.743556	31.015847
498.681622	29553.388791	31.020864
498.785441	29578.501419	31.025882
499.469991	29604.398306	31.030900
499.864846	29667.817091	31.035917
500.374238	29698.894589	31.040935
500.918863	29735.304005	31.045952
500.738098	29779.820928	31.050970
501.511615	29804.630832	31.055988
501.692672	29858.224123	31.061005
502.100176	29899.776581	31.066023
502.585176	29952.506049	31.071040
502.963038	30004.351127	31.076058
503.317279	30048.591084	31.081076
503.648408	30111.416304	31.086093
504.355098	30153.897916	31.091111
504.788754	30224.442019	31.096128
505.244991	30281.994535	31.101146
505.778220	30337.771008	31.106164
505.938663	30399.631705	31.111181
506.367489	30444.156895	31.116199
507.204145	30499.230725	31.121216
507.443063	30566.483219	31.126234
508.328695	30611.021718	31.131252
508.495007	30681.545573	31.136269
509.215208	30728.480974	31.141287
509.632076	30794.966721	31.146304
509.698926	30866.053537	31.151322
510.682429	30914.378255	31.156340
511.015230	30979.641879	31.161357
511.706026	31045.938210	31.166375
511.887885	31095.626247	31.171392
512.305424	31164.776027	31.176410
513.686315	31211.120894	31.181428
514.274088	31281.631185	31.186445
515.068301	31327.839800	31.191463
515.191270	31364.962715	31.196480
515.258506	31422.706278	31.201498
516.010841	31483.548635	31.206516
516.585294	31545.215640	31.211533
517.021987	31581.536310	31.216551
517.504342	31625.582415	31.221568
517.506304	31680.905102	31.226586
518.466422	31733.782316	31.231604
518.643542	31783.962111	31.236621
519.656226	31844.166417	31.241639
520.051489	31892.531051	31.246656
520.393239	31949.375983	31.251674
520.847022	31993.008106	31.256692
521.000996	32060.870355	31.261709
522.020942	32121.743290	31.266727
522.364174	32171.243650	31.271744
522.755210	32236.555963	31.276762
523.214196	32292.899910	31.281780
524.026013	32358.143174	31.286797
524.125393	32421.923626	31.291815
525.090276	32473.707446	31.296832
525.668414	32542.290278	31.301850
526.202113	32592.678515	31.306868
526.565876	32660.233920	31.311885
526.879896	32717.628603	31.316903
528.013780	32781.138520	31.321920
528.081177	32848.065224	31.326938
528.665155	32900.317080	31.331956
529.130596	32966.695740	31.336973
530.364141	33018.856436	31.341991
532.215756	33043.666413	31.347008
532.959575	33085.943909	31.352026
533.579348	33116.860945	31.357044
534.150254	33144.747580	31.362061
534.314896	33184.022496	31.367079
534.439240	33223.237894	31.372096
534.898675	33263.158458	31.377114
535.355827	33303.029004	31.382132
536.132124	33355.323015	31.387149
536.234160	33402.329798	31.392167
536.413158	33460.550646	31.397184
536.884337	33513.005955	31.402202
537.366707	33558.880675	31.407220
537.984087	33622.494707	31.412237
538.026726	33675.238996	31.417255
538.606852	33732.586711	31.422272
538.822749	33805.121696	31.427290
539.321294	33855.702354	31.432308
540.041037	33927.170136	31.437325
540.409892	33993.287767	31.442343
540.890557	34055.805759	31.447360
541.497236	34135.815882	31.452378
542.114693	34196.308067	31.457396
543.017180	34258.059744	31.462413
543.578916	34318.564704	31.467431
544.260378	34378.163402	31.472448
544.490737	34439.013808	31.477466
545.064890	34500.981491	31.482484
545.968396	34557.704156	31.487501
546.497916	34616.448358	31.492519
547.278207	34673.150721	31.497536
547.562457	34739.493366	31.502554
548.267932	34792.260867	31.507572
549.205307	34832.806560	31.512589
549.625363	34894.157326	31.517607
550.522768	34941.172501	31.522624
550.680850	34998.237425	31.527642
551.585032	35040.739236	31.532660
551.873314	35089.654105	31.537677
552.484058	35137.080039	31.542695
553.197885	35172.598653	31.547712
553.129486	35221.228829	31.552730
553.756533	35275.721074	31.557748
554.189418	35326.591301	31.562765
554.541480	35381.021993	31.567783
555.207987	35431.913891	31.572800
555.286631	35486.775056	31.577818
555.930716	35545.310900	31.582836
556.457136	35610.720567	31.587853
556.775311	35685.060844	31.592871
557.757320	35728.441355	31.597888
558.214055	35790.593854	31.602906
559.235011	35838.338900	31.607924
559.941127	35889.579005	31.612941
560.527574	35960.780321	31.617959
560.948806	36002.521600	31.622976
561.486477	36059.530372	31.627994
562.252038	36109.776684	31.633012
562.669999	36170.687212	31.638029
562.751302	36238.766764	31.643047
563.372220	36301.168474	31.648064
563.748045	36359.849120	31.653082
564.109121	36425.396369	31.658100
564.898799	36487.644621	31.663117
565.567010	36539.694436	31.668135
566.527588	36598.869432	31.673152
567.367844	36665.584990	31.678170
567.869570	36722.343023	31.683188
568.461926	36779.849997	31.688205
569.101319	36830.895524	31.693223
570.052317	36871.099603	31.698240
570.580386	36924.988341	31.703258
570.924219	36986.519820	31.708276
571.680798	37028.899254	31.713293
572.516515	37070.770230	31.718311
573.378043	37114.723140	31.723328
574.201641	37167.468673	31.728346
574.461410	37211.767374	31.733364
575.068903	37254.837878	31.738381
575.460763	37301.399925	31.743399
576.218324	37339.131134	31.748416
576.397831	37392.832674	31.753434
576.989424	37445.001915	31.758452
577.688143	37498.154078	31.763469
577.886417	37547.526049	31.768487
578.555294	37609.665585	31.773504
578.849434	37658.406594	31.778522
579.037613	37719.085738	31.783540
579.863933	37781.799519	31.788557
580.072038	37844.214798	31.793575
580.714307	37901.830732	31.798592
581.225327	37972.029889	31.803610
582.009671	38049.515878	31.808628
582.451933	38115.355700	31.813645
582.687799	38190.625737	31.818663
583.492061	38248.799912	31.823680
583.899333	38319.614069	31.828698
584.720191	38382.662236	31.833716
585.453310	38446.482604	31.838733
585.568567	38524.279973	31.843751
586.159245	38590.501006	31.848768
586.723652	38669.392621	31.853786
587.191497	38742.464608	31.858804
588.031258	38807.070322	31.863821
588.318496	38891.519523	31.868839
589.022035	38965.225768	31.873856
590.084412	39031.452569	31.878874
590.894841	39100.135807	31.883892
591.586681	39155.348740	31.888909
591.817609	39222.641520	31.893927
592.623053	39281.652089	31.898944
592.973528	39337.988802	31.903962
593.143251	39400.482057	31.908980
594.108262	39460.385356	31.913997
594.309459	39534.738713	31.919015
594.805876	39592.014808	31.924032
595.708781	39666.372753	31.929050
596.182943	39729.918446	31.934068
596.911421	39796.225275	31.939085
597.392881	39872.825297	31.944103
598.058894	39946.939431	31.949120
598.574122	40023.146261	31.954138
598.778817	40092.529860	31.959156
599.637559	40161.998248	31.964173
599.840513	40239.608539	31.969191
600.430110	40321.921661	31.974208
601.472878	40387.007658	31.979226
601.982960	40467.838370	31.984244
602.331357	40528.636158	31.989261
603.290838	40613.130664	31.994279
604.154632	40690.469583	31.999296
604.869693	40766.147765	32.004314
605.402228	40829.899135	32.009332
606.601512	40891.460393	32.014349
607.127518	40957.609167	32.019367
607.748021	41013.893826	32.024384
608.542577	41076.437977	32.029402
609.072502	41136.020897	32.034420
609.825376	41205.851656	32.039437
610.339707	41273.581839	32.044455
611.209342	41322.654295	32.049472
612.184161	41387.505696	32.054490
612.897437	41439.442173	32.059508
613.556600	41492.268463	32.064525
614.116738	41555.275965	32.069543
614.656613	41600.931211	32.074560
615.077479	41661.019987	32.079578
615.368097	41732.772642	32.084596
616.166019	41784.048976	32.089613
616.352666	41846.970792	32.094631
617.317205	41899.826740	32.099648
617.920451	41969.388374	32.104666
618.386905	42029.871740	32.109684
618.861917	42097.987116	32.114701
619.152179	42177.475808	32.119719
619.730888	42236.167163	32.124736
620.399077	42318.949789	32.129754
621.111794	42386.960680	32.134772
621.478057	42447.742926	32.139789
621.841796	42530.071677	32.144807
622.351129	42603.843590	32.149824
623.028919	42693.972469	32.154842
623.596080	42780.562174	32.159860
624.481956	42850.964401	32.164877
624.876421	42924.273547	32.169895
625.447728	42998.365124	32.174912
626.016177	43079.664904	32.179930
627.049905	43163.022342	32.184948
627.899356	43228.608102	32.189965
628.470604	43312.386708	32.194983
629.412057	43386.286111	32.200000
630.064867	43449.325815	32.205018
630.519146	43523.044184	32.210036
631.555470	43593.253906	32.215053
632.039647	43668.944256	32.220071
632.414208	43724.220177	32.225088
633.209160	43801.848724	32.230106
633.606458	43870.902183	32.235124
634.235377	43919.389878	32.240141
634.672899	43981.952332	32.245159
635.361831	44055.605647	32.250176
636.646137	44114.524244	32.255194
637.012472	44184.995241	32.260212
637.697021	44232.091716	32.265229
637.930799	44315.785349	32.270247
638.434568	44382.423642	32.275264
639.275491	44445.217810	32.280282
639.613184	44519.814995	32.285300
640.786801	44585.055230	32.290317
640.769419	44670.531584	32.295335
641.369821	44745.825087	32.300352
641.725864	44818.974400	32.305370
642.415219	44906.248436	32.310388
643.794170	44968.927098	32.315405
644.192511	45041.394630	32.320423
644.505856	45122.720211	32.325440
645.661067	45197.380844	32.330458
646.216913	45270.748360	32.335476
647.287578	45340.346472	32.340493
647.775760	45416.595798	32.345511
648.274428	45498.359700	32.350528
649.092246	45568.297215	32.355546
649.967621	45653.715870	32.360564
650.118591	45729.886390	32.365581
650.857573	45785.941802	32.370599
651.169182	45867.845561	32.375616
652.167472	45943.671779	32.380634
652.722992	46035.456814	32.385652
653.276032	46101.297402	32.390669
653.898353	46182.901778	32.395687
654.430270	46264.145690	32.400704
655.369694	46331.779910	32.405722
655.938543	46419.996588	32.410740
657.002608	46496.344648	32.415757
657.833791	46567.502505	32.420775
658.674476	46639.284269	32.425792
659.321125	46708.177557	32.430810
659.481602	46788.007310	32.435828
660.814447	46852.897606	32.440845
661.417444	46938.275513	32.445863
662.147238	46997.954730	32.450880
663.272096	47057.319436	32.455898
663.541093	47131.161559	32.460916
664.008857	47197.705284	32.465933
664.570421	47274.969962	32.470951
665.007014	47346.104352	32.475968
666.117823	47417.683427	32.480986
666.094902	47494.631865	32.486004
667.029442	47561.469240	32.491021
667.533436	47648.199279	32.496039
667.990084	47724.257904	32.501056
668.687198	47805.869581	32.506074
669.549388	47886.045965	32.511092
670.191776	47949.806728	32.516109
670.817322	48036.695309	32.521127
671.302303	48127.977969	32.526144
672.143493	48199.904526	32.531162
673.092849	48292.743904	32.536180
673.498186	48363.520962	32.541197
674.130961	48438.997578	32.546215
674.923450	48515.900759	32.551232
675.638507	48594.013894	32.556250
676.247896	48675.710117	32.561268
676.814509	48764.083360	32.566285
677.356366	48838.698665	32.571303
677.500343	48921.044393	32.576320
678.352200	48996.348089	32.581338
679.160027	49081.989202	32.586356
679.409622	49156.846657	32.591373
680.297114	49238.868857	32.596391
681.029515	49323.806638	32.601408
681.730297	49404.107666	32.606426
682.336217	49484.389959	32.611444
683.024917	49573.261557	32.616461
683.557712	49664.199451	32.621479
684.086114	49756.843889	32.626496
684.808706	49840.538130	32.631514
685.036021	49928.884371	32.636532
686.457681	50025.020781	32.641549
686.960990	50119.442848	32.646567
687.659678	50218.772536	32.651584
688.769619	50304.375553	32.656602
689.154877	50394.141157	32.661620
689.924842	50481.171779	32.666637
691.100905	50546.801731	32.671655
691.720388	50640.935571	32.676672
692.912551	50712.703105	32.681690
693.656243	50800.115347	32.686708
694.076062	50868.524255	32.691725
695.224718	50946.016378	32.696743
695.940431	51030.632862	32.701760
696.817263	51104.993236	32.706778
697.171716	51184.758834	32.711796
697.571531	51254.900040	32.716813
698.649568	51329.367022	32.721831
699.566869	51413.361281	32.726848
699.905474	51493.986701	32.731866
699.962066	51582.258189	32.736884
700.603543	51670.919891	32.741901
701.527724	51752.975214	32.746919
702.312972	51861.995534	32.751936
702.915437	51936.139112	32.756954
703.871101	52016.680605	32.761972
704.008284	52104.097849	32.766989
705.104042	52194.597830	32.772007
705.464626	52290.664958	32.777024
705.911347	52393.130200	32.782042
706.955878	52487.941963	32.787060
707.457386	52585.042240	32.792077
708.119173	52671.099339	32.797095
708.839552	52775.258637	32.802112
709.731607	52869.642606	32.807130
710.676983	52969.034160	32.812148
711.107327	53057.196946	32.817165
712.256395	53139.372625	32.822183
712.967478	53232.884864	32.827200
713.995903	53318.145151	32.832218
714.472813	53413.093075	32.837236
715.128152	53503.374974	32.842253
715.988822	53599.517609	32.847271
716.414210	53688.985479	32.852288
717.287183	53777.362720	32.857306
717.854481	53877.882701	32.862324
718.707729	53974.590676	32.867341
719.410332	54053.040734	32.872359
720.170847	54138.171958	32.877376
720.729482	54226.912710	32.882394
721.341041	54333.884420	32.887412
722.382473	54422.369434	32.892429
723.366742	54494.747606	32.897447
723.985308	54590.480220	32.902464
724.420248	54679.729924	32.907482
725.034313	54761.678580	32.912500
725.787441	54854.850479	32.917517
726.412616	54933.714883	32.922535
726.873650	55024.661370	32.927552
727.432511	55119.010155	32.932570
728.185792	55210.850624	32.937588
728.691986	55310.231849	32.942605
729.398108	55404.033286	32.947623
729.808819	55494.390039	32.952640
730.598182	55592.613942	32.957658
731.456814	55702.205927	32.962676
732.118444	55800.009686	32.967693
732.803870	55899.149467	32.972711
733.597641	56012.608016	32.977728
734.594535	56111.185649	32.982746
736.038238	56186.128922	32.987764
736.797089	56286.692788	32.992781
737.763039	56372.905489	32.997799
738.178197	56471.423027	33.002816
739.612816	56553.148863	33.007834
740.723921	56640.280211	33.012852
741.214146	56726.535103	33.017869
741.624832	56799.566188	33.022887
742.233407	56886.427767	33.027904
742.570753	56976.948745	33.032922
743.213684	57071.362487	33.037940
743.664169	57179.014426	33.042957
744.809657	57287.759049	33.047975
745.559062	57379.054200	33.052992
746.088889	57483.149890	33.058010
747.430517	57567.024687	33.063028
748.024790	57664.406469	33.068045
748.716299	57760.995455	33.073063
749.214584	57867.038243	33.078080
749.715956	57974.319591	33.083098
750.384519	58068.455805	33.088116
751.167134	58195.925124	33.093133
751.652123	58289.050063	33.098151
752.417941	58397.718112	33.103168
753.385718	58503.528780	33.108186
753.839554	58624.849806	33.113204
754.389757	58744.942379	33.118221
755.226294	58865.531840	33.123239
756.184735	58971.453952	33.128256
756.726992	59077.710758	33.133274
757.615340	59197.642780	33.138292
757.993779	59320.724594	33.143309
759.206734	59429.368643	33.148327
760.073762	59555.739436	33.153344
760.744608	59660.391924	33.158362
761.652141	59768.393106	33.163380
762.220890	59892.552903	33.168397
763.520918	60006.595194	33.173415
764.252378	60107.486193	33.178432
764.886615	60222.890927	33.183450
766.193243	60324.730773	33.188468
766.815272	60428.599042	33.193485
768.559309	60519.598926	33.198503
769.063158	60601.179068	33.203520
769.993647	60696.049049	33.208538
771.028377	60784.651995	33.213556
771.549229	60884.911765	33.218573
772.523839	60971.768551	33.223591
773.215598	61067.355920	33.228608
773.772554	61151.280506	33.233626
774.336302	61239.621945	33.238644
775.089002	61332.065818	33.243661
776.618570	61405.662048	33.248679
777.662808	61497.028377	33.253696
777.859063	61574.030671	33.258714
779.026919	61649.760488	33.263732
779.189533	61738.100818	33.268749
779.992155	61798.255627	33.273767
780.837513	61891.318759	33.278784
780.852440	61982.073544	33.283802
781.854481	62066.775322	33.288820
782.339631	62167.647744	33.293837
783.092227	62256.954700	33.298855
783.637182	62356.882788	33.303872
783.903335	62462.728967	33.308890
784.716082	62568.795133	33.313908
785.042109	62681.742943	33.318925
785.980036	62798.578513	33.323943
786.531329	62919.928189	33.328960
787.030900	63043.088464	33.333978
788.015196	63165.290887	33.338996
788.520332	63289.937051	33.344013
789.317574	63417.297841	33.349031
790.266474	63544.084484	33.354048
790.923052	63681.595809	33.359066
791.908136	63800.565702	33.364084
792.529160	63932.181027	33.369101
793.628614	64052.580949	33.374119
794.439400	64179.444889	33.379136
795.595068	64314.115830	33.384154
796.486510	64417.890418	33.389172
797.303547	64544.098199	33.394189
798.247704	64674.792625	33.399207
798.666928	64788.204385	33.404224
800.162045	64918.992691	33.409242
801.121085	65027.164964	33.414260
801.848346	65149.250954	33.419277
802.569634	65267.925221	33.424295
803.754534	65387.332729	33.429312
803.973461	65512.368305	33.434330
805.059481	65617.766639	33.439348
805.697856	65730.053794	33.444365
806.727048	65857.473538	33.449383
807.770801	65982.982602	33.454400
807.985619	66101.947558	33.459418
809.048762	66212.479364	33.464436
809.466070	66333.801720	33.469453
810.512319	66451.563054	33.474471
811.070650	66584.937708	33.479488
811.771409	66723.915929	33.484506
812.605986	66845.741309	33.489524
813.245062	66985.313048	33.494541
813.883880	67111.053819	33.499559
814.982317	67242.510190	33.504576
815.568864	67372.806517	33.509594
816.750900	67506.305330	33.514612
817.695542	67643.011459	33.519629
818.486841	67768.914340	33.524647
819.563274	67897.312324	33.529664
820.369364	68024.959162	33.534682
821.611813	68139.719950	33.539700
822.071518	68255.375584	33.544717
823.213716	68377.532084	33.549735
824.410988	68486.599687	33.554752
825.435997	68595.298002	33.559770
826.356989	68706.372238	33.564788
827.112692	68825.048399	33.569805
827.790123	68926.592138	33.574823
828.980690	69030.365602	33.579840
829.900883	69136.928114	33.584858
831.247627	69239.911818	33.589876
832.077666	69340.642057	33.594893
832.389076	69426.676581	33.599911
833.127617	69516.244723	33.604928
833.921556	69617.329975	33.609946
834.536174	69710.491603	33.614964
834.851175	69814.754908	33.619981
835.375449	69930.971767	33.624999
836.228018	70041.729225	33.630016
836.840294	70155.561805	33.635034
837.476880	70273.494397	33.640052
837.968545	70398.684754	33.645069
838.826928	70517.764426	33.650087
840.125366	70648.652616	33.655104
840.836794	70772.645493	33.660122
841.480955	70898.635578	33.665140
842.250230	71024.049333	33.670157
843.096500	71153.845552	33.675175
843.784849	71283.889940	33.680192
844.244820	71423.558519	33.685210
845.456376	71548.333252	33.690228
846.357811	71678.838056	33.695245
846.932291	71817.067600	33.700263
848.487538	71945.101220	33.705280
849.453102	72081.921062	33.710298
850.499921	72215.718494	33.715316
851.571553	72330.479571	33.720333
852.996014	72462.629043	33.725351
854.016969	72574.889435	33.730368
854.747961	72692.851401	33.735386
855.479473	72802.195102	33.740404
856.172776	72912.671242	33.745421
857.073939	73047.206125	33.750439
857.806416	73168.218372	33.755456
858.047783	73288.351206	33.760474
859.260894	73411.100317	33.765492
860.380186	73539.613804	33.770509
861.067918	73660.965028	33.775527
862.122863	73788.972080	33.780544
862.599545	73927.724563	33.785562
863.556713	74053.580276	33.790580
864.272922	74189.537713	33.795597
864.699626	74320.712369	33.800615
865.824802	74447.889612	33.805632
866.481793	74591.713631	33.810650
867.102905	74736.973745	33.815668
867.906897	74874.919352	33.820685
868.564830	75029.484305	33.825703
869.578268	75168.971885	33.830720
870.463421	75311.580372	33.835738
871.047698	75468.222266	33.840756
872.401589	75617.547546	33.845773
873.431353	75753.127779	33.850791
874.592313	75888.718812	33.855808
875.410316	76027.409328	33.860826
876.317962	76173.574010	33.865844
877.655106	76303.408612	33.870861
878.560562	76440.278509	33.875879
880.141119	76554.130401	33.880896
881.155309	76683.482992	33.885914
882.225454	76788.199184	33.890932
883.362366	76904.194279	33.895949
884.179043	77022.899211	33.900967
884.960055	77137.113824	33.905984
885.389814	77250.008237	33.911002
886.629795	77367.247369	33.916020
887.514890	77477.955302	33.921037
888.131339	77609.472499	33.926055
889.239352	77715.584627	33.931072
889.896775	77828.532953	33.936090
890.780987	77929.414438	33.941108
892.245467	78023.565720	33.946125
893.473165	78123.354088	33.951143
894.723726	78216.826793	33.956160
895.396277	78305.771744	33.961178
895.746720	78399.261010	33.966196
896.655749	78508.015706	33.971213
897.298291	78608.054671	33.976231
898.035434	78702.474405	33.981248
898.877209	78816.384040	33.986266
899.543295	78930.348566	33.991284
900.313638	79037.661306	33.996301
901.459976	79153.976567	34.001319
902.159005	79270.347313	34.006336
902.980239	79395.262972	34.011354
903.397421	79523.940050	34.016372
904.265679	79641.436004	34.021389
904.458344	79785.598264	34.026407
905.747246	79913.886964	34.031424
906.066527	80050.635553	34.036442
906.881365	80196.152593	34.041460
907.662986	80342.580620	34.046477
908.384784	80502.398187	34.051495
909.207723	80655.975725	34.056512
910.619801	80800.202515	34.061530
911.224504	80946.151298	34.066548
911.928518	81110.549641	34.071565
912.899239	81270.426445	34.076583
914.041690	81424.772501	34.081600
914.760574	81586.337852	34.086618
916.059698	81740.546330	34.091636
917.197419	81902.576168	34.096653
917.895268	82053.647128	34.101671
918.731801	82197.750128	34.106688
920.187686	82343.725544	34.111706
921.004290	82503.807306	34.116724
922.268865	82640.061225	34.121741
923.362516	82796.790689	34.126759
924.153992	82939.944240	34.131776
925.207366	83099.972122	34.136794
925.784675	83235.855947	34.141812
927.130389	83388.568560	34.146829
928.061360	83545.001048	34.151847
928.600972	83689.706584	34.156864
929.791342	83842.504814	34.161882
931.018401	83975.242678	34.166900
932.068603	84121.435636	34.171917
933.245221	84274.314935	34.176935
934.626343	84396.679353	34.181952
935.631431	84534.316018	34.186970
936.978554	84651.271706	34.191988
938.481718	84773.396544	34.197005
939.060967	84903.064337	34.202023
939.803297	85018.261647	34.207040
940.901375	85146.725291	34.212058
941.266198	85277.961706	34.217076
942.429260	85397.096408	34.222093
942.550927	85535.024094	34.227111
943.612123	85674.765201	34.232128
944.342842	85825.988464	34.237146
944.860918	85977.665414	34.242164
945.759806	86113.285352	34.247181
946.719608	86263.815620	34.252199
948.102096	86407.177885	34.257216
948.711467	86546.625529	34.262234
949.500321	86699.085029	34.267252
950.698126	86842.315955	34.272269
951.250440	87003.592580	34.277287
952.084650	87154.231594	34.282304
952.990223	87298.671495	34.287322
953.734452	87444.062748	34.292340
954.560047	87585.537351	34.297357
955.137663	87738.582679	34.302375
956.538340	87886.506919	34.307392
958.338920	88016.230873	34.312410
958.950108	88164.034099	34.317428
960.426642	88294.040888	34.322445
961.218736	88437.690259	34.327463
962.438247	88589.939099	34.332480
962.988509	88720.316317	34.337498
964.028029	88871.843676	34.342516
965.463849	89001.367516	34.347533
965.753389	89147.888488	34.352551
966.772836	89299.137142	34.357568
968.028001	89445.759986	34.362586
968.407906	89596.185896	34.367604
969.655939	89736.034295	34.372621
970.309543	89900.136402	34.377639
970.938153	90055.067811	34.382656
972.137969	90222.878915	34.387674
972.904889	90392.129594	34.392692
973.740916	90548.371577	34.397709
974.756999	90712.963683	34.402727
975.653614	90894.397712	34.407744
976.428075	91066.816165	34.412762
977.365490	91240.215199	34.417780
978.444401	91406.149689	34.422797
979.547194	91584.719698	34.427815
980.554227	91741.004526	34.432832
981.927722	91907.273571	34.437850
983.360216	92084.508132	34.442868
985.529740	92214.700431	34.447885
987.431844	92346.513469	34.452903
988.757289	92463.093879	34.457920
990.354744	92591.648553	34.462938
991.225272	92726.817427	34.467956
991.956434	92839.978876	34.472973
993.190815	92969.601814	34.477991
993.948739	93082.880233	34.483008
994.500197	93204.433723	34.488026
995.141093	93341.878109	34.493044
996.279438	93468.051219	34.498061
996.996958	93598.079309	34.503079
997.703110	93737.496196	34.508096
998.861711	93861.016064	34.513114
999.362337	94020.886663	34.518132
1000.373620	94167.097598	34.523149
1001.162418	94315.599394	34.528167
1002.626513	94455.635798	34.533184
1003.458022	94588.897344	34.538202
1004.414901	94743.798375	34.543220
1005.268358	94883.032927	34.548237
1006.230622	95029.953368	34.553255
1006.537090	95193.389253	34.558272
1007.213495	95356.663877	34.563290
1008.368264	95524.196442	34.568308
1009.332927	95669.113807	34.573325
1010.138993	95834.262783	34.578343
1011.216985	96006.280115	34.583360
1012.837422	96164.239133	34.588378
1014.137110	96328.506039	34.593396
1015.529954	96476.174262	34.598413
1016.446189	96630.353291	34.603431
1016.961188	96787.277110	34.608448
1018.164427	96928.706308	34.613466
1018.952606	97097.183620	34.618484
1019.815894	97240.702675	34.623501
1021.217774	97383.563931	34.628519
1021.924515	97530.275581	34.633536
1022.542378	97676.559652	34.638554
1023.542894	97832.605982	34.643572
1024.513366	97985.043644	34.648589
1025.302410	98142.500501	34.653607
1026.388475	98303.897458	34.658624
1027.547633	98453.166957	34.663642
1028.318841	98623.107054	34.668660
1029.209319	98790.186213	34.673677
1030.172686	98959.368857	34.678695
1030.920198	99135.140442	34.683712
1032.147703	99308.491677	34.688730
1032.931256	99492.742869	34.693748
1033.952328	99677.785522	34.698765
1035.047710	99850.459588	34.703783
1035.955581	100035.112049	34.708800
1037.032872	100207.525649	34.713818
1037.845059	100401.743527	34.718836
1038.300566	100597.066385	34.723853
1039.599917	100782.520677	34.728871
1041.273662	100968.402009	34.733888
1042.605124	101146.705901	34.738906
1043.697044	101336.092103	34.743924
1044.787973	101513.545581	34.748941
1045.819660	101700.405625	34.753959
1046.425442	101892.693612	34.758976
1047.621037	102079.212802	34.763994
1048.853439	102270.975986	34.769012
1049.615867	102465.287446	34.774029
1050.557352	102658.551448	34.779047
1051.571182	102861.485856	34.784064
1052.849859	103046.586430	34.789082
1054.090172	103243.883027	34.794100
1055.396102	103431.273910	34.799117
1056.605136	103613.395174	34.804135
1057.464001	103816.957860	34.809152
1058.962639	103998.521153	34.814170
1060.196294	104186.771570	34.819188
1061.242030	104369.007418	34.824205
1062.345936	104546.536646	34.829223
1063.683252	104729.714669	34.834240
1064.728128	104909.769915	34.839258
1065.583871	105098.285607	34.844276
1066.446224	105275.834350	34.849293
1067.648490	105472.514618	34.854311
1068.539955	105662.814151	34.859328
1069.890489	105848.948648	34.864346
1070.763929	106040.482353	34.869364
1071.395465	106221.786332	34.874381
1072.685362	106418.015957	34.879399
1073.248841	106623.029732	34.884416
1074.618243	106811.067654	34.889434
1075.606540	107016.926236	34.894452
1076.455629	107222.834730	34.899469
1077.748948	107420.033788	34.904487
1078.996501	107620.458866	34.909504
1080.588401	107791.077503	34.914522
1081.825121	107979.930883	34.919540
1083.030605	108156.239145	34.924557
1084.510120	108334.187874	34.929575
1085.206320	108527.466030	34.934592
1086.731239	108705.029764	34.939610
1087.733717	108866.633172	34.944628
1088.476067	109064.796645	34.949645
1090.094649	109247.984905	34.954663
1090.888864	109433.400426	34.959680
1091.713446	109589.629087	34.964698
1092.910471	109759.020849	34.969716
1094.075988	109918.197065	34.974733
1094.981484	110082.851077	34.979751
1095.771443	110264.029737	34.984768
1096.787740	110450.112253	34.989786
1097.856362	110620.341286	34.994804
1099.092091	110778.092300	34.999821
1100.492596	110958.288141	35.004839
1102.224301	111122.900761	35.009856
1103.433477	111280.899756	35.014874
1104.171009	111455.584157	35.019892
1105.363383	111622.087567	35.024909
1107.171422	111777.469807	35.029927
1107.607877	111951.117695	35.034944
1108.693453	112124.127497	35.039962
1109.716376	112296.946056	35.044980
1110.531312	112477.083921	35.049997
1111.933973	112660.102861	35.055015
1112.500532	112843.096360	35.060032
1113.641048	113009.477422	35.065050
1114.643254	113200.926863	35.070068
1115.528724	113392.118207	35.075085
1116.602222	113583.520530	35.080103
1117.704569	113786.320817	35.085120
1118.580374	113972.007088	35.090138
1119.793446	114178.605131	35.095156
1119.907374	114392.847899	35.100173
1121.107295	114600.971473	35.105191
1122.170412	114824.346959	35.110208
1123.331816	115025.828999	35.115226
1124.206053	115250.784669	35.120244
1125.635443	115470.392875	35.125261
1127.460225	115662.128894	35.130279
1129.540666	115865.378305	35.135296
1130.862465	116062.913890	35.140314
1132.499669	116251.910337	35.145332
1133.564054	116447.223300	35.150349
1134.498363	116624.188291	35.155367
1135.343342	116828.548134	35.160384
1136.457773	117034.245971	35.165402
1137.440744	117230.578693	35.170420
1138.565574	117422.467572	35.175437
1139.477339	117624.351504	35.180455
1140.347478	117834.048491	35.185472
1141.577647	118056.674491	35.190490
1142.451701	118247.964153	35.195508
1143.508993	118467.276951	35.200525
1144.466431	118671.935559	35.205543
1145.492824	118897.237189	35.210560
1146.826044	119115.660476	35.215578
1148.178919	119332.675729	35.220596
1149.196895	119568.690766	35.225613
1151.007012	119765.626592	35.230631
1151.628481	119992.878930	35.235648
1152.723823	120202.226595	35.240666
1153.770105	120407.579777	35.245684
1154.992134	120634.547945	35.250701
1156.365378	120846.933511	35.255719
1157.161493	121078.917289	35.260736
1157.786002	121296.004124	35.265754
1159.383954	121520.902366	35.270772
1160.217834	121755.292898	35.275789
1160.984819	121976.656993	35.280807
1162.363570	122208.984399	35.285824
1163.735567	122433.141276	35.290842
1165.744616	122646.803537	35.295860
1167.164621	122869.004295	35.300877
1168.534724	123079.277618	35.305895
1169.457937	123273.088686	35.310912
1170.676514	123458.551779	35.315930
1171.718440	123653.245485	35.320948
1172.436000	123869.005298	35.325965
1173.584798	124066.662149	35.330983
1174.479033	124273.828946	35.336000
1175.756651	124507.052830	35.341018
1177.108803	124718.531965	35.346036
1177.629383	124936.372363	35.351053
1179.227369	125153.060662	35.356071
1180.018356	125365.143913	35.361088
1180.943745	125601.121185	35.366106
1182.219250	125834.913364	35.371124
1183.152016	126064.543616	35.376141
1185.387999	126289.207861	35.381159
1186.269616	126525.706525	35.386176
1187.493269	126749.362616	35.391194
1189.122691	126971.305759	35.396212
1189.456020	127192.678663	35.401229
1190.967070	127422.388488	35.406247
1192.385320	127655.562759	35.411264
1193.257787	127890.451211	35.416282
1194.270954	128131.059768	35.421300
1195.379923	128374.911756	35.426317
1197.054537	128596.783178	35.431335
1198.062709	128824.330414	35.436352
1199.954454	129052.823519	35.441370
1201.738448	129285.962449	35.446388
1202.735584	129516.659982	35.451405
1203.878266	129735.014988	35.456423
1204.983355	129961.464514	35.461440
1205.831724	130199.657365	35.466458
1206.926948	130423.450058	35.471476
1208.084723	130673.155411	35.476493
1209.482696	130906.382859	35.481511
1211.114372	131137.786193	35.486528
1212.186783	131364.796318	35.491546
1213.605671	131595.401540	35.496564
1214.697920	131840.462257	35.501581
1215.767567	132074.107471	35.506599
1217.356708	132304.677088	35.511616
1218.155237	132556.320042	35.516634
1219.422583	132777.984100	35.521652
1220.702639	133007.012609	35.526669
1221.905618	133244.979758	35.531687
1223.148809	133485.502717	35.536704
1224.430106	133722.319592	35.541722
1226.291508	133931.432387	35.546740
1227.873702	134154.752706	35.551757
1229.541454	134373.002342	35.556775
1231.268939	134592.295791	35.561792
1232.512226	134804.026333	35.566810
1233.808509	134997.025258	35.571828
1234.706068	135216.181021	35.576845
1236.092627	135428.868148	35.581863
1237.184472	135643.633704	35.586880
1238.185043	135856.374654	35.591898
1239.417107	136060.356571	35.596916
1240.375789	136279.927758	35.601933
1241.307913	136505.044998	35.606951
1242.515206	136728.647729	35.611968
1243.641210	136957.133739	35.616986
1244.382333	137179.624747	35.622004
1245.673239	137410.749075	35.627021
1247.315114	137631.167372	35.632039
1248.319612	137871.571946	35.637056
1249.148319	138101.902579	35.642074
1250.424181	138321.663204	35.647092
1251.676500	138540.643093	35.652109
1252.641260	138772.857694	35.657127
1253.852994	138991.644379	35.662144
1254.569007	139221.088462	35.667162
1255.911134	139456.744875	35.672180
1256.786907	139689.576418	35.677197
1257.889497	139938.487274	35.682215
1259.509525	140179.313986	35.687232
1261.074305	140422.598635	35.692250
1262.402828	140654.271676	35.697268
1263.664371	140916.109126	35.702285
1264.826497	141151.769015	35.707303
1266.035807	141399.075343	35.712320
1266.861480	141658.860251	35.717338
1267.831792	141916.733957	35.722356
1268.714035	142177.236202	35.727373
1269.694029	142438.738687	35.732391
1271.077504	142714.974276	35.737408
1272.334106	143004.623346	35.742426
1273.824932	143270.473212	35.747444
1275.477918	143543.006301	35.752461
1276.407702	143819.173395	35.757479
1277.654828	144099.043766	35.762496
1279.143349	144375.769752	35.767514
1280.259485	144657.580996	35.772532
1281.301748	144944.555154	35.777549
1282.561927	145228.046436	35.782567
1284.150543	145504.308254	35.787584
1285.629724	145790.240718	35.792602
1287.278625	146078.151127	35.797620
1289.313260	146345.963509	35.802637
1290.325214	146608.417540	35.807655
1292.314724	146871.308192	35.812672
1293.645594	147141.804379	35.817690
1295.561366	147393.982292	35.822708
1296.895557	147655.807435	35.827725
1297.786374	147913.395773	35.832743
1299.789002	148161.214787	35.837760
1301.301049	148423.333182	35.842778
1302.638151	148653.890824	35.847796
1303.756412	148901.264780	35.852813
1304.959071	149157.402726	35.857831
1306.384505	149407.316626	35.862848
1307.689626	149663.390468	35.867866
1308.582467	149914.575204	35.872884
1309.793618	150175.069009	35.877901
1311.158644	150433.116827	35.882919
1312.608050	150680.321271	35.887936
1313.631603	150957.136459	35.892954
1314.825112	151211.793575	35.897972
1316.097938	151482.521671	35.902989
1317.236059	151748.885530	35.908007
1318.774865	151998.569890	35.913024
1319.894185	152256.810397	35.918042
1321.546810	152517.311119	35.923060
1322.959738	152783.383279	35.928077
1324.252699	153052.102647	35.933095
1325.797652	153303.494250	35.938112
1327.272248	153568.572402	35.943130
1328.640780	153809.938112	35.948148
1330.076727	154086.226220	35.953165
1331.606693	154331.310388	35.958183
1332.829604	154582.471823	35.963200
1334.179553	154838.522773	35.968218
1335.785342	155070.635735	35.973236
1337.299490	155322.375459	35.978253
1338.055462	155576.017790	35.983271
1339.495460	155800.843480	35.988288
1340.871677	156051.354912	35.993306
1341.727053	156283.535546	35.998324
1343.440123	156519.318050	36.003341
1344.448330	156761.598844	36.008359
1345.895694	156987.711325	36.013376
1346.739762	157248.542380	36.018394
1347.942738	157495.463671	36.023412
1349.415271	157736.988824	36.028429
1350.615470	157998.577903	36.033447
1351.844143	158248.239678	36.038464
1352.763958	158527.016548	36.043482
1353.896968	158787.150365	36.048500
1355.139341	159046.417878	36.053517
1356.500704	159321.994035	36.058535
1357.943358	159597.698205	36.063552
1359.062619	159886.029418	36.068570
1360.262808	160166.610832	36.073588
1361.304409	160461.872851	36.078605
1362.788529	160752.547677	36.083623
1364.562073	161042.263388	36.088640
1366.223282	161326.557214	36.093658
1367.854294	161594.149871	36.098676
1370.758428	161842.631158	36.103693
1372.452186	162100.333904	36.108711
1373.848410	162356.793310	36.113728
1374.782611	162627.641270	36.118746
1376.195866	162886.968352	36.123764
1377.328654	163146.127651	36.128781
1378.017260	163424.227502	36.133799
1379.919889	163693.514273	36.138816
1381.440242	163962.396428	36.143834
1382.403964	164235.444778	36.148852
1383.446569	164517.172724	36.153869
1384.721845	164800.145572	36.158887
1386.490680	165070.693862	36.163904
1387.731350	165366.033845	36.168922
1389.052765	165645.985020	36.173940
1390.305685	165927.852491	36.178957
1391.500095	166227.634064	36.183975
1392.741578	166525.823948	36.188992
1393.848134	166834.886440	36.194010
1395.323693	167134.082285	36.199028
1396.684478	167423.567242	36.204045
1398.049401	167730.309544	36.209063
1399.690042	168027.428734	36.214080
1401.322357	168332.139020	36.219098
1403.022323	168623.669490	36.224116
1404.476550	168924.606663	36.229133
1405.701605	169226.446523	36.234151
1406.909839	169516.401757	36.239168
1408.869643	169827.450707	36.244186
1410.073795	170134.946698	36.249204
1411.248773	170419.266628	36.254221
1412.050715	170740.473880	36.259239
1413.490716	171041.046873	36.264256
1414.959565	171358.671568	36.269274
1416.257612	171677.075329	36.274292
1417.614991	171994.101035	36.279309
1418.516648	172320.188372	36.284327
1419.551774	172628.845710	36.289344
1421.178459	172961.619585	36.294362
1422.139364	173300.520708	36.299380
1423.783247	173629.108838	36.304397
1424.978995	173949.867314	36.309415
1426.851138	174291.975382	36.314432
1428.422062	174625.112873	36.319450
1429.824767	174956.300767	36.324468
1430.978027	175273.230030	36.329485
1432.471041	175591.602800	36.334503
1434.362505	175912.132775	36.339520
1435.781126	176231.575368	36.344538
1436.997290	176547.563523	36.349556
1438.606305	176864.491476	36.354573
1439.833303	177188.819873	36.359591
1441.523158	177492.210044	36.364608
1442.743249	177815.807644	36.369626
1443.453961	178147.398011	36.374644
1445.720491	178465.395358	36.379661
1447.151785	178793.342959	36.384679
1448.840697	179114.587213	36.389696
1450.279949	179430.607758	36.394714
1451.596498	179757.451053	36.399732
1453.022570	180081.207008	36.404749
1454.302862	180420.891817	36.409767
1455.742981	180752.861275	36.414784
1456.889174	181094.806449	36.419802
1458.188533	181448.037176	36.424820
1460.055018	181784.308972	36.429837
1461.645913	182135.440163	36.434855
1463.070509	182477.323138	36.439872
1464.904916	182803.465710	36.444890
1466.276975	183146.669024	36.449908
1467.952098	183477.601701	36.454925
1469.174691	183841.281763	36.459943
1470.481763	184187.421820	36.464960
1471.797239	184538.106724	36.469978
1473.280762	184889.756222	36.474996
1474.714589	185234.536661	36.480013
1476.390829	185612.255635	36.485031
1477.981506	185964.490979	36.490048
1480.085857	186310.957296	36.495066
1481.715406	186650.192849	36.500084
1484.045750	186979.261751	36.505101
1485.909311	187309.488565	36.510119
1487.977708	187626.000003	36.515136
1489.707457	187937.415546	36.520154
1491.008268	188259.629667	36.525172
1492.327075	188573.299825	36.530189
1493.772689	188896.991524	36.535207
1495.247557	189207.288278	36.540224
1497.058783	189518.534024	36.545242
1498.850810	189831.929894	36.550260
1500.525447	190137.057653	36.555277
1501.876727	190436.908867	36.560295
1503.517430	190746.704143	36.565312
1505.182043	191047.674645	36.570330
1506.238074	191366.239803	36.575348
1507.673628	191678.980824	36.580365
1508.781760	191994.582982	36.585383
1510.281575	192321.915335	36.590400
1511.457869	192636.316350	36.595418
1512.661817	192963.827965	36.600436
1514.149249	193294.011232	36.605453
1515.269353	193628.890485	36.610471
1516.134429	193976.216484	36.615488
1517.707198	194324.087802	36.620506
1518.818215	194676.797881	36.625524
1520.293427	195018.455971	36.630541
1521.658241	195387.784071	36.635559
1523.143708	195744.462735	36.640576
1524.549383	196098.173197	36.645594
1526.240337	196460.547542	36.650612
1527.428236	196821.254988	36.655629
1529.076177	197195.459994	36.660647
1530.719962	197544.035575	36.665664
1532.670783	197877.086432	36.670682
1533.890146	198230.839350	36.675700
1535.722635	198572.698670	36.680717
1537.000241	198921.113478	36.685735
1538.773060	199261.983234	36.690752
1540.578351	199591.105642	36.695770
1541.327499	199946.684626	36.700788
1542.630633	200287.662480	36.705805
1544.382667	200640.057959	36.710823
1546.407045	200987.700033	36.715840
1548.172136	201333.152110	36.720858
1550.021045	201692.253314	36.725876
1552.091088	202020.454997	36.730893
1554.206446	202355.849621	36.735911
1556.057240	202675.914047	36.740928
1558.108346	202993.344077	36.745946
1558.901446	203326.180936	36.750964
1560.861801	203658.864830	36.755981
1562.167564	203996.140215	36.760999
1563.432512	204331.671750	36.766016
1564.511682	204675.805851	36.771034
1565.681026	205020.739289	36.776052
1567.253196	205373.353018	36.781069
1568.846244	205730.904120	36.786087
1570.143043	206095.857425	36.791104
1571.551834	206452.820213	36.796122
1572.731906	206832.194901	36.801140
1574.380060	207201.285635	36.806157
1575.563215	207579.482669	36.811175
1576.159027	207971.186913	36.816192
1578.345411	208356.459713	36.821210
1579.704920	208760.434615	36.826228
1581.142900	209161.440094	36.831245
1582.819339	209561.405127	36.836263
1584.183905	209975.302212	36.841280
1586.053507	210373.182367	36.846298
1587.705317	210794.172372	36.851316
1589.288040	211200.027325	36.856333
1590.786090	211610.101259	36.861351
1592.184511	212026.568049	36.866368
1593.710048	212433.441556	36.871386
1595.573709	212848.235655	36.876404
1597.203915	213266.473396	36.881421
1599.041332	213692.424913	36.886439
1600.726570	214110.327470	36.891456
1602.383625	214521.481109	36.896474
1603.531426	214947.374685	36.901492
1605.367183	215370.591667	36.906509
1606.927692	215793.957625	36.911527
1608.510766	216228.471215	36.916544
1610.557555	216647.925877	36.921562
1611.939727	217080.419406	36.926580
1613.738888	217497.480561	36.931597
1615.361071	217916.807741	36.936615
1617.078995	218353.950229	36.941632
1619.026883	218821.737466	36.946650
1620.848666	219231.259167	36.951668
1622.425286	219645.115296	36.956685
1624.941068	220036.518497	36.961703
1626.338049	220451.347311	36.966720
1628.718163	220841.887051	36.971738
1630.842735	221226.374776	36.976756
1632.722509	221604.630840	36.981773
1634.237676	221982.567438	36.986791
1635.549194	222371.358880	36.991808
1637.391891	222747.796408	36.996826
1638.797737	223150.036517	37.001844
1639.840218	223535.498443	37.006861
1641.398281	223903.605192	37.011879
1642.332412	224280.832834	37.016896
1644.733448	224636.103260	37.021914
1647.091164	224995.115655	37.026932
1649.005507	225356.564472	37.031949
1650.440825	225716.747265	37.036967
1651.640441	226086.977514	37.041984
1652.954802	226440.629348	37.047002
1654.517450	226837.293950	37.052020
1655.809322	227219.678972	37.057037
1657.279768	227583.442930	37.062055
1659.436832	227962.715700	37.067072
1661.243071	228342.682495	37.072090
1663.514194	228698.138727	37.077108
1665.349316	229060.017940	37.082125
1667.371297	229418.641484	37.087143
1668.776581	229792.277791	37.092160
1670.492882	230160.580527	37.097178
1671.966860	230544.266179	37.102196
1673.365580	230925.069651	37.107213
1675.176029	231279.160913	37.112231
1676.194277	231687.487380	37.117248
1677.992335	232076.483330	37.122266
1679.559817	232469.277701	37.127284
1681.156662	232860.569624	37.132301
1682.946876	233249.011160	37.137319
1684.282745	233657.062100	37.142336
1685.835873	234060.023451	37.147354
1687.204745	234475.666060	37.152372
1688.770907	234894.858796	37.157389
1690.297726	235296.328964	37.162407
1691.430110	235725.781364	37.167424
1693.735551	236161.798138	37.172442
1695.296427	236592.655354	37.177460
1696.803360	237021.515819	37.182477
1698.750814	237446.570609	37.187495
1700.676815	237878.971055	37.192512
1702.728723	238301.826081	37.197530
1704.454001	238729.562312	37.202548
1706.069149	239168.291309	37.207565
1707.506555	239581.140614	37.212583
1708.993785	240023.829946	37.217600
1710.523115	240464.252520	37.222618
1712.642347	240908.643059	37.227636
1714.551780	241337.345194	37.232653
1716.776111	241767.850596	37.237671
1718.509654	242198.412408	37.242688
1720.626724	242632.595108	37.247706
1722.800985	243050.156032	37.252724
1724.706746	243463.570590	37.257741
1726.800962	243864.990201	37.262759
1728.590924	244283.581948	37.267776
1730.296558	244701.222999	37.272794
1732.236532	245099.697906	37.277812
1733.596151	245522.579465	37.282829
1735.349173	245931.831746	37.287847
1736.587235	246353.820119	37.292864
1738.027031	246771.914603	37.297882
1739.666847	247196.759210	37.302900
1741.468283	247631.713455	37.307917
1743.396916	248044.597637	37.312935
1744.681229	248485.353968	37.317952
1746.012863	248913.249185	37.322970
1748.261671	249352.018479	37.327988
1750.071151	249776.025436	37.333005
1751.814305	250206.826399	37.338023
1753.337572	250644.726136	37.343040
1755.071455	251080.914981	37.348058
1756.786945	251502.348108	37.353076
1757.933611	251914.171479	37.358093
1759.743834	252324.564770	37.363111
1760.946435	252759.674264	37.368128
1762.706707	253190.246558	37.373146
1764.851367	253610.518286	37.378164
1766.245385	254047.985081	37.383181
1767.879653	254483.253262	37.388199
1769.511628	254919.131771	37.393216
1771.361415	255355.381051	37.398234
1772.760502	255804.736779	37.403252
1774.442955	256259.964943	37.408269
1775.890802	256725.926792	37.413287
1777.337363	257198.366881	37.418304
1778.893696	257665.073293	37.423322
1780.760516	258146.767376	37.428340
1782.368126	258635.007589	37.433357
1784.286754	259126.626039	37.438375
1785.698195	259622.545179	37.443392
1787.522594	260112.121620	37.448410
1789.640444	260595.121013	37.453428
1792.577340	261075.114702	37.458445
1795.065429	261538.035157	37.463463
1797.073004	262008.325565	37.468480
1799.153307	262485.335758	37.473498
1801.483780	262941.880318	37.478516
1803.352317	263418.188490	37.483533
1805.051029	263871.128094	37.488551
1806.772290	264330.033567	37.493568
1808.357021	264795.185151	37.498586
1810.371529	265262.348666	37.503604
1811.650842	265756.433593	37.508621
1813.040576	266230.761693	37.513639
1814.667444	266718.742665	37.518656
1816.353824	267210.701744	37.523674
1818.713578	267689.771554	37.528692
1820.312301	268175.012434	37.533709
1822.714819	268652.981997	37.538727
1824.645929	269138.954617	37.543744
1826.297644	269620.197044	37.548762
1828.418599	270093.232575	37.553780
1829.764568	270581.637202	37.558797
1831.723732	271061.379284	37.563815
1833.640964	271556.750472	37.568832
1835.628732	272034.632168	37.573850
1838.001591	272512.729116	37.578868
1839.439187	273003.655665	37.583885
1841.226421	273485.632820	37.588903
1843.203388	273981.295403	37.593920
1844.990013	274463.931583	37.598938
1847.039302	274939.487095	37.603956
1848.686618	275442.187279	37.608973
1850.964511	275922.402861	37.613991
1852.952059	276404.443633	37.619008
1854.557119	276890.255343	37.624026
1856.794023	277368.010917	37.629044
1858.251844	277852.371653	37.634061
1860.542008	278329.583048	37.639079
1862.678529	278800.137992	37.644096
1864.408000	279270.632069	37.649114
1866.594925	279747.146174	37.654132
1868.270708	280227.807846	37.659149
1869.877955	280711.375529	37.664167
1872.222434	281181.763829	37.669184
1874.260341	281654.284526	37.674202
1876.219083	282109.493066	37.679220
1878.077958	282577.824287	37.684237
1879.789643	283040.259996	37.689255
1881.627460	283494.138760	37.694272
1882.996006	283941.006722	37.699290
1884.835904	284386.347895	37.704308
1885.982722	284851.132720	37.709325
1887.899052	285309.032552	37.714343
1889.574786	285772.254258	37.719360
1891.000283	286247.606885	37.724378
1892.838401	286733.050474	37.729396
1894.439756	287218.480791	37.734413
1896.062996	287703.118516	37.739431
1897.523174	288206.578226	37.744448
1899.471001	288711.759227	37.749466
1901.682350	289200.435321	37.754484
1903.165948	289719.558117	37.759501
1905.065274	290234.825722	37.764519
1906.892504	290753.125925	37.769536
1908.363057	291292.108030	37.774554
1910.289991	291815.645516	37.779572
1911.948691	292345.600565	37.784589
1913.599110	292888.457986	37.789607
1915.093872	293439.822300	37.794624
1917.298458	293999.829992	37.799642
1919.698613	294546.214019	37.804660
1921.604957	295105.046577	37.809677
1923.796308	295657.759001	37.814695
1926.339269	296193.698042	37.819712
1928.136387	296757.442696	37.824730
1930.363410	297293.149242	37.829748
1932.683711	297849.055356	37.834765
1934.838639	298392.896078	37.839783
1936.878542	298934.594128	37.844800
1938.435370	299486.528501	37.849818
1940.355404	300038.323850	37.854836
1942.320817	300598.210801	37.859853
1944.192555	301145.842816	37.864871
1946.423267	301688.307627	37.869888
1948.378692	302245.190046	37.874906
1950.727713	302801.801180	37.879924
1952.413547	303363.191628	37.884941
1954.149117	303924.621345	37.889959
1956.691123	304467.679458	37.894976
1958.728721	305016.557325	37.899994
1961.101248	305560.246467	37.905012
1963.227590	306113.039595	37.910029
1965.144600	306655.730566	37.915047
1967.367568	307191.739250	37.920064
1969.102569	307738.567764	37.925082
1970.887896	308289.143138	37.930100
1972.889845	308845.723467	37.935117
1974.892275	309391.430623	37.940135
1977.380136	309923.746809	37.945152
1979.606676	310462.832460	37.950170
1982.071547	310988.949010	37.955188
1984.382645	311513.843124	37.960205
1986.578014	312031.769246	37.965223
1989.193067	312542.309038	37.970240
1991.021633	313059.019145	37.975258
1993.590210	313561.560593	37.980276
1995.241062	314081.873775	37.985293
1997.007559	314591.168650	37.990311
1999.425753	315075.745818	37.995328
2001.217745	315578.046429	38.000346
2003.283088	316069.328485	38.005364
2005.145772	316581.793434	38.010381
2006.400327	317103.775974	38.015399
2008.501456	317616.524366	38.020416
2009.857951	318147.674784	38.025434
2011.413143	318641.156408	38.030452
2013.386962	319155.590543	38.035469
2014.996196	319662.920348	38.040487
2017.157177	320164.035897	38.045504
2018.683926	320675.967788	38.050522
2020.939759	321180.132625	38.055540
2022.886330	321706.765461	38.060557
2024.480099	322233.477706	38.065575
2026.540773	322750.028432	38.070592
2028.532509	323288.321133	38.075610
2030.044168	323818.258805	38.080628
2032.035268	324356.238016	38.085645
2034.169691	324908.255298	38.090663
2036.444748	325460.803145	38.095680
2037.829527	326016.666687	38.100698
2039.721726	326570.435786	38.105716
2041.728440	327136.545673	38.110733
2043.374171	327714.515825	38.115751
2045.189275	328291.487746	38.120768
2046.714535	328881.551718	38.125786
2048.767751	329472.132089	38.130804
2050.664550	330085.378608	38.135821
2052.534824	330692.453810	38.140839
2054.510198	331298.819855	38.145856
2056.426485	331921.564108	38.150874
2058.605353	332536.185153	38.155892
2061.270726	333158.157613	38.160909
2063.500075	333784.815424	38.165927
2065.914262	334396.813202	38.170944
2067.885122	335027.307502	38.175962
2069.927205	335650.167077	38.180980
2072.481458	336268.797204	38.185997
2074.391021	336900.422149	38.191015
2076.533808	337517.887205	38.196032
2078.376656	338151.640579	38.201050
2080.575657	338782.459143	38.206068
2082.860277	339417.088894	38.211085
2084.185103	340055.727424	38.216103
2086.647927	340686.326886	38.221120
2088.751560	341329.821502	38.226138
2091.509961	341957.488090	38.231156
2093.333432	342593.271009	38.236173
2095.507958	343238.226903	38.241191
2098.087257	343870.340639	38.246208
2100.023561	344524.430885	38.251226
2102.302171	345146.678921	38.256244
2104.338570	345780.227835	38.261261
2106.309718	346428.753452	38.266279
2108.529968	347072.660723	38.271296
2110.235001	347717.633944	38.276314
2112.314653	348369.921817	38.281332
2114.716771	349020.878381	38.286349
2116.275396	349686.379807	38.291367
2118.555730	350339.596392	38.296384
2120.665257	351002.094600	38.301402
2122.643726	351648.743803	38.306420
2125.734707	352303.371563	38.311437
2128.466667	352934.042563	38.316455
2131.071015	353556.655913	38.321472
2133.792906	354188.655473	38.326490
2136.213844	354807.068795	38.331508
2138.638928	355428.898216	38.336525
2140.125865	356053.182431	38.341543
2142.311451	356664.731182	38.346560
2144.019381	357287.615950	38.351578
2146.096369	357917.535260	38.356596
2148.536389	358537.971701	38.361613
2149.767018	359165.651978	38.366631
2151.482482	359780.099770	38.371648
2153.004061	360395.915046	38.376666
2155.144223	361028.897179	38.381684
2157.174629	361641.235206	38.386701
2159.026752	362267.902548	38.391719
2161.056795	362889.228271	38.396736
2163.072405	363539.646257	38.401754
2164.838589	364179.109551	38.406772
2166.876125	364820.344267	38.411789
2168.663210	365472.163209	38.416807
2170.644456	366134.923724	38.421824
2172.672819	366809.106047	38.426842
2175.000329	367485.307300	38.431860
2177.278207	368154.934615	38.436877
2179.120200	368840.095618	38.441895
2181.744400	369516.338410	38.446912
2183.792281	370208.669770	38.451930
2185.971273	370890.516079	38.456948
2188.759732	371564.386168	38.461965
2190.971292	372267.406515	38.466983
2193.612004	372944.750383	38.472000
2195.905595	373630.534076	38.477018
2198.007800	374315.854346	38.482036
2200.704154	374987.443875	38.487053
2202.776738	375685.144891	38.492071
2205.379577	376371.636372	38.497088
2207.686797	377055.069132	38.502106
2209.411528	377747.004208	38.507124
2211.544196	378441.064518	38.512141
2213.579967	379158.964651	38.517159
2215.764945	379854.965800	38.522176
2218.212563	380562.827830	38.527194
2220.156398	381251.587624	38.532212
2222.550955	381955.245157	38.537229
2224.412455	382685.422868	38.542247
2226.963002	383389.252635	38.547264
2229.438455	384108.774941	38.552282
2231.758201	384820.624580	38.557300
2234.660308	385509.746429	38.562317
2237.151037	386216.466468	38.567335
2239.412076	386914.385922	38.572352
2241.511596	387617.970547	38.577370
2244.152963	388326.901083	38.582388
2246.665517	389017.482359	38.587405
2249.183659	389724.069588	38.592423
2251.464759	390408.853110	38.597440
2254.213445	391095.800686	38.602458
2256.492211	391777.233672	38.607476
2258.605575	392454.496336	38.612493
2260.760780	393148.847378	38.617511
2262.981617	393845.579891	38.622528
2265.467435	394536.068038	38.627546
2267.498992	395223.066811	38.632564
2269.682648	395912.939645	38.637581
2271.695248	396611.138137	38.642599
2273.952351	397302.867705	38.647616
2276.103110	397997.006393	38.652634
2278.598130	398690.793213	38.657652
2281.321185	399375.427857	38.662669
2283.431148	400063.467425	38.667687
2285.608930	400753.532227	38.672704
2287.385210	401465.161557	38.677722
2289.234629	402167.841316	38.682740
2292.020712	402868.905011	38.687757
2294.027006	403584.700891	38.692775
2296.316727	404283.683025	38.697792
2298.790868	404988.546567	38.702810
2300.852086	405701.619184	38.707828
2303.577320	406388.365770	38.712845
2305.918020	407072.093106	38.717863
2308.716058	407735.231590	38.722880
2311.107831	408381.294589	38.727898
2313.803622	409042.188907	38.732916
2316.261089	409688.716890	38.737933
2318.388369	410361.554511	38.742951
2320.366809	411014.463179	38.747968
2323.094674	411667.511109	38.752986
2325.730093	412307.208732	38.758004
2328.043710	412957.583021	38.763021
2330.790559	413613.493266	38.768039
2332.911452	414279.495628	38.773056
2335.166672	414932.743918	38.778074
2337.346022	415594.144157	38.783092
2339.351235	416245.020082	38.788109
2341.445523	416920.229592	38.793127
2343.164676	417595.002160	38.798144
2345.534590	418279.678735	38.803162
2347.490517	418983.956171	38.808180
2349.912336	419673.651929	38.813197
2351.775998	420387.225165	38.818215
2353.435802	421099.672397	38.823232
2356.464309	421810.557095	38.828250
2358.647385	422539.184740	38.833268
2360.897079	423268.565108	38.838285
2362.896660	424009.182046	38.843303
2364.789812	424751.186947	38.848320
2367.021165	425510.380875	38.853338
2368.740592	426283.611012	38.858356
2370.940025	427047.927315	38.863373
2373.314653	427831.025766	38.868391
2375.670100	428622.101612	38.873408
2378.757597	429397.285301	38.878426
2380.994373	430188.278521	38.883444
2383.567563	430972.760650	38.888461
2386.117320	431756.815738	38.893479
2388.584031	432541.870947	38.898496
2391.509113	433318.218956	38.903514
2394.101565	434112.261920	38.908532
2396.634057	434899.049525	38.913549
2398.998874	435681.181513	38.918567
2401.100357	436480.285895	38.923584
2403.632425	437272.205901	38.928602
2405.459624	438077.221432	38.933620
2408.064447	438874.995200	38.938637
2410.312418	439673.558830	38.943655
2412.783185	440485.315835	38.948672
2415.742433	441275.153272	38.953690
2418.460569	442091.163174	38.958708
2421.253097	442877.075146	38.963725
2424.092348	443672.716805	38.968743
2426.504545	444454.334686	38.973760
2430.017558	445234.427850	38.978778
2432.207185	446003.581192	38.983796
2434.870403	446777.081226	38.988813
2437.275198	447548.168058	38.993831
2439.319662	448326.014765	38.998848
2441.919779	449090.994448	39.003866
2443.997304	449887.191917	39.008884
2446.545229	450659.509152	39.013901
2448.971275	451441.377832	39.018919
2450.990224	452227.887252	39.023936
2453.346791	453009.102412	39.028954
2455.444258	453813.746635	39.033972
2457.647844	454605.396123	39.038989
2459.787590	455401.425557	39.044007
2461.840023	456205.327330	39.049024
2464.362578	457003.861473	39.054042
2466.599557	457787.647114	39.059060
2469.329868	458561.866386	39.064077
2472.066308	459342.071839	39.069095
2474.177913	460118.507926	39.074112
2477.423006	460882.543382	39.079130
2479.960471	461654.502361	39.084148
2482.303188	462433.844324	39.089165
2484.892840	463205.886540	39.094183
2487.324474	464006.888850	39.099200
2489.439046	464783.497388	39.104218
2491.397081	465573.545885	39.109236
2493.616604	466381.512456	39.114253
2496.219496	467194.436485	39.119271
2498.220519	468004.595759	39.124288
2500.397886	468825.961619	39.129306
2502.439764	469665.304834	39.134324
2504.852837	470491.715410	39.139341
2507.661758	471339.297842	39.144359
2510.101491	472209.337389	39.149376
2512.452720	473061.718784	39.154394
2514.874533	473926.731264	39.159412
2517.591789	474793.373087	39.164429
2520.153019	475667.174156	39.169447
2522.415169	476534.972471	39.174464
2525.196120	477409.110504	39.179482
2528.044453	478296.884559	39.184500
2530.365032	479164.701899	39.189517
2533.202193	480052.039814	39.194535
2535.532740	480937.953730	39.199552
2538.623079	481817.336367	39.204570
2541.387056	482704.305003	39.209588
2543.633574	483591.366013	39.214605
2546.495726	484484.038147	39.219623
2548.843526	485380.234574	39.224640
2552.181031	486260.218259	39.229658
2554.134301	487162.549837	39.234676
2557.263513	488038.743934	39.239693
2560.098509	488913.933494	39.244711
2563.095740	489811.515515	39.249728
2565.407228	490705.328515	39.254746
2567.841872	491585.346886	39.259764
2569.932679	492480.871804	39.264781
2573.179998	493369.699960	39.269799
2574.982376	494273.708646	39.274816
2577.578918	495170.625567	39.279834
2580.407688	496072.906887	39.284852
2582.335162	496983.664920	39.289869
2585.194742	497897.550483	39.294887
2587.256229	498818.884182	39.299904
2589.748421	499728.291525	39.304922
2592.446629	500671.565822	39.309940
2594.798512	501605.512027	39.314957
2597.212495	502535.663053	39.319975
2599.555748	503484.687641	39.324992
2602.476469	504415.759142	39.330010
2605.149464	505367.899250	39.335028
2607.513029	506310.554459	39.340045
2610.408382	507256.244418	39.345063
2612.621429	508211.874737	39.350080
2615.595934	509160.314804	39.355098
2618.479823	510116.377420	39.360116
2621.455019	511049.984315	39.365133
2624.585377	511982.049259	39.370151
2627.564298	512937.474013	39.375168
2630.649659	513855.776050	39.380186
2633.840700	514758.735506	39.385204
2636.626263	515663.272454	39.390221
2639.697928	516560.755446	39.395239
2642.005219	517443.295679	39.400256
2644.047306	518310.914024	39.405274
2646.588692	519183.490822	39.410292
2648.674945	520058.310419	39.415309
2651.061262	520951.017420	39.420327
2653.314750	521848.682038	39.425344
2655.774436	522734.774289	39.430362
2658.862425	523631.592202	39.435380
2661.464843	524528.538021	39.440397
2664.480858	525424.204150	39.445415
2667.254523	526319.957846	39.450432
2669.539910	527212.364509	39.455450
2672.037291	528113.244079	39.460468
2675.037617	529022.697934	39.465485
2678.320110	529907.477836	39.470503
2681.815210	530804.002035	39.475520
2684.827921	531683.534367	39.480538
2687.669642	532582.474900	39.485556
2689.492962	533471.510606	39.490573
2692.460815	534380.287517	39.495591
2695.041777	535279.306820	39.500608
2697.471665	536184.184155	39.505626
2700.157443	537090.070030	39.510644
2702.590481	538002.784876	39.515661
2705.717218	538923.378914	39.520679
2708.239495	539847.485434	39.525696
2711.685698	540744.763415	39.530714
2715.025180	541648.039857	39.535732
2717.750403	542563.484395	39.540749
2720.474113	543465.287571	39.545767
2722.757067	544392.709402	39.550784
2725.252416	545313.948918	39.555802
2727.869850	546235.258618	39.560820
2729.968181	547168.964888	39.565837
2732.683895	548104.970891	39.570855
2734.809669	549070.377410	39.575872
2737.314531	550024.994336	39.580890
2739.857088	551002.365075	39.585908
2741.788508	551982.129826	39.590925
2744.186816	552974.114032	39.595943
2746.067054	553986.871677	39.600960
2748.780385	554995.495951	39.605978
2751.335193	556010.353577	39.610996
2753.906821	557036.389280	39.616013
2757.582560	558059.049009	39.621031
2760.402092	559101.217606	39.626048
2763.146148	560141.458149	39.631066
2765.686229	561184.263326	39.636084
2768.089874	562237.357444	39.641101
2770.854204	563280.814179	39.646119
2773.553077	564348.107334	39.651136
2776.357033	565402.941088	39.656154
2779.105513	566467.943503	39.661172
2781.914168	567534.304968	39.666189
2785.017722	568600.278940	39.671207
2787.872071	569673.536155	39.676224
2790.177054	570745.338397	39.681242
2793.398070	571834.569967	39.686260
2796.099551	572921.334627	39.691277
2799.199161	573976.170299	39.696295
2802.552289	575062.945261	39.701312
2804.841114	576140.719133	39.706330
2807.591766	577210.848084	39.711348
2811.063493	578286.336019	39.716365
2813.932571	579345.475556	39.721383
2817.101822	580421.431082	39.726400
2820.628850	581463.225580	39.731418
2824.790255	582475.737074	39.736436
2827.669252	583474.484478	39.741453
2830.876031	584454.892810	39.746471
2833.791357	585434.267701	39.751488
2836.781850	586407.384299	39.756506
2839.300447	587378.495304	39.761524
2841.654005	588354.067563	39.766541
2844.540948	589311.878181	39.771559
2846.986488	590291.890293	39.776576
2849.074788	591286.566386	39.781594
2851.908632	592276.175710	39.786612
2854.308463	593287.773377	39.791629
2857.049315	594289.858725	39.796647
2859.548216	595314.445510	39.801664
2862.309040	596346.214636	39.806682
2865.366831	597372.584513	39.811700
2867.703966	598413.008484	39.816717
2870.590872	599462.164472	39.821735
2873.118771	600508.029954	39.826752
2875.625082	601569.678984	39.831770
2878.612283	602633.354589	39.836788
2881.378965	603719.098030	39.841805
2884.226904	604795.864619	39.846823
2887.191003	605884.324462	39.851840
2890.064863	606964.787180	39.856858
2893.413752	608047.821728	39.861876
2896.589772	609140.339614	39.866893
2900.149033	610223.882098	39.871911
2903.658321	611302.925722	39.876928
2906.933449	612396.012343	39.881946
2910.918711	613447.605679	39.886964
2913.630600	614505.812245	39.891981
2917.268311	615558.514110	39.896999
2921.256221	616580.302411	39.902016
2924.893759	617613.155119	39.907034
2928.031733	618647.643364	39.912052
2930.370168	619679.816180	39.917069
2933.182520	620714.613155	39.922087
2935.967249	621743.068366	39.927104
2938.045479	622787.936761	39.932122
2940.470488	623841.243416	39.937140
2943.249305	624901.435247	39.942157
2946.577611	625948.690808	39.947175
2948.984390	627001.192254	39.952192
2951.130862	628068.620348	39.957210
2954.406411	629145.396495	39.962228
2957.079513	630227.507369	39.967245
2959.900346	631307.585852	39.972263
2963.180354	632400.961335	39.977280
2965.911871	633488.372066	39.982298
2969.446146	634575.837660	39.987316
2972.268728	635669.897300	39.992333
2975.050562	636751.070703	39.997351
2978.148676	637851.395203	40.002368
2980.938263	638958.141658	40.007386
2984.437292	640040.950448	40.012404
2988.110523	641130.502396	40.017421
2991.829861	642194.437828	40.022439
2995.240800	643253.574694	40.027456
2998.492090	644322.753647	40.032474
3001.797186	645378.295772	40.037492
3004.723096	646439.126733	40.042509
3007.657292	647485.235268	40.047527
3010.486695	648552.093601	40.052544
3012.890911	649603.255161	40.057562
3016.015769	650667.846329	40.062580
3018.859980	651743.036888	40.067597
3021.391756	652816.169687	40.072615
3024.069148	653878.399174	40.077632
3026.871922	654927.639107	40.082650
3030.352901	655952.094153	40.087668
3032.807293	656986.525428	40.092685
3035.925886	658022.432123	40.097703
3038.528705	659061.103570	40.102720
3041.705311	660094.938805	40.107738
3044.659069	661148.220879	40.112756
3047.381813	662211.086180	40.117773
3050.018987	663273.799368	40.122791
3052.628210	664357.705656	40.127808
3055.207422	665449.707629	40.132826
3057.833245	666541.229573	40.137844
3060.854107	667658.189347	40.142861
3063.142465	668778.074896	40.147879
3066.926981	669900.219101	40.152896
3069.229736	671034.960610	40.157914
3072.538755	672179.596671	40.162932
3075.881079	673316.230901	40.167949
3079.082789	674467.519618	40.172967
3083.031837	675609.992228	40.177984
3085.977441	676755.920906	40.183002
3089.257311	677905.630365	40.188020
3092.170088	679074.591957	40.193037
3095.303600	680240.288754	40.198055
3098.554731	681406.167009	40.203072
3101.192501	682581.239744	40.208090
3104.477525	683753.422755	40.213108
3107.510182	684938.560422	40.218125
3110.458627	686131.355253	40.223143
3112.972802	687320.341126	40.228160
3115.656463	688545.933883	40.233178
3118.708281	689759.733135	40.238196
3121.873430	690989.482171	40.243213
3124.477222	692231.910259	40.248231
3127.789920	693455.738570	40.253248
3130.640034	694709.195277	40.258266
3133.958752	695961.306955	40.263284
3137.726842	697219.516970	40.268301
3140.706395	698470.784298	40.273319
3143.996792	699716.070730	40.278336
3147.133677	700986.541707	40.283354
3150.375743	702243.327232	40.288372
3153.497326	703505.751030	40.293389
3156.646485	704782.012439	40.298407
3159.940057	706057.368674	40.303424
3163.204163	707323.623786	40.308442
3166.225887	708592.110692	40.313460
3169.806022	709871.363563	40.318477
3173.200349	711135.946032	40.323495
3176.663371	712398.993071	40.328512
3180.154880	713676.799370	40.333530
3183.414440	714932.077449	40.338548
3187.828268	716192.819311	40.343565
3191.015437	717437.640471	40.348583
3194.619705	718663.357443	40.353600
3198.387338	719890.698730	40.358618
3201.929921	721108.894454	40.363636
3205.720028	722326.525130	40.368653
3209.083286	723541.575213	40.373671
3212.493781	724735.673598	40.378688
3216.197109	725929.402817	40.383706
3219.534757	727099.738676	40.388724
3223.245949	728282.497992	40.393741
3226.206014	729452.115560	40.398759
3229.248654	730620.761517	40.403776
3232.160165	731797.758123	40.408794
3234.823402	732968.846134	40.413812
3238.123800	734126.869020	40.418829
3240.826560	735271.393374	40.423847
3243.692616	736409.704871	40.428864
3246.045383	737559.935156	40.433882
3248.749828	738725.884737	40.438900
3251.728491	739885.302163	40.443917
3254.040855	741066.470096	40.448935
3257.124936	742254.883589	40.453952
3259.806713	743464.001393	40.458970
3262.419232	744684.289165	40.463988
3265.142987	745921.086471	40.469005
3267.838496	747177.070339	40.474023
3271.271723	748427.308598	40.479040
3274.001635	749715.661124	40.484058
3276.492959	751000.045138	40.489076
3279.879420	752306.241571	40.494093
3282.815592	753633.672042	40.499111
3285.745897	754955.161442	40.504128
3288.910719	756318.047618	40.509146
3291.627896	757674.561270	40.514164
3294.986546	759051.306081	40.519181
3297.998118	760418.556654	40.524199
3301.319156	761808.540764	40.529216
3304.741986	763211.734104	40.534234
3308.305199	764614.348156	40.539252
3312.043572	766025.918184	40.544269
3314.840553	767452.227983	40.549287
3319.246682	768856.908812	40.554304
3322.784520	770270.168163	40.559322
3326.127744	771679.701135	40.564340
3329.892411	773091.549555	40.569357
3333.128954	774530.283733	40.574375
3336.624084	775939.321513	40.579392
3340.533539	777371.100902	40.584410
3343.879468	778791.890815	40.589428
3347.055365	780217.634926	40.594445
3350.346440	781654.220974	40.599463
3353.943065	783079.038290	40.604480
3357.177445	784516.830814	40.609498
3360.742541	785939.026817	40.614516
3364.641130	787355.098883	40.619533
3368.401281	788793.908243	40.624551
3372.588981	790197.061690	40.629568
3376.601028	791600.211717	40.634586
3379.669476	793008.531044	40.639604
3383.689168	794405.634452	40.644621
3387.191399	795797.941240	40.649639
3391.920575	797160.875911	40.654656
3395.380064	798532.469242	40.659674
3399.236311	799887.670707	40.664692
3402.837449	801238.685434	40.669709
3406.280724	802589.952032	40.674727
3409.809800	803944.315937	40.679744
3413.427062	805283.871300	40.684762
3416.592462	806627.152195	40.689780
3420.008818	807959.957948	40.694797
3423.339618	809302.245942	40.699815
3426.936733	810642.025969	40.704832
3430.512326	811968.399913	40.709850
3433.270732	813303.784836	40.714868
3436.616437	814626.303859	40.719885
3439.950908	815975.083831	40.724903
3442.477629	817321.089048	40.729920
3446.048573	818676.317549	40.734938
3448.909420	820037.830400	40.739956
3452.278800	821405.763810	40.744973
3455.563934	822776.941731	40.749991
3458.437414	824159.658648	40.755008
3461.842608	825521.603494	40.760013
3464.041176	826854.207127	40.765018
3467.569097	828124.643558	40.770023
3470.221063	829360.577410	40.775028
3472.983589	830529.181269	40.780032
3475.890024	831642.208501	40.785037
3479.409334	832685.886227	40.790042
3482.512116	833654.557262	40.795047
3485.018842	834557.707731	40.800052
3487.643004	835394.515102	40.805056
3490.131438	836178.470108	40.810061
3491.999766	836900.984064	40.815066
3494.467770	837533.083528	40.820071
3496.239488	838132.394682	40.825076
3498.624881	838670.313221	40.830080
3500.492566	839138.649052	40.835085
3501.859451	839553.172774	40.840090
3503.646429	839944.281824	40.845095
3504.957503	840289.493696	40.850100
3506.064300	840580.625048	40.855104
3507.344472	840821.376911	40.860109
3507.929408	841046.869995	40.865114
3509.167689	841228.497496	40.870119
3509.936156	841374.203023	40.875124
3511.237160	841499.626020	40.880128
3512.031378	841581.870170	40.885133
3512.550887	841633.237934	40.890138
3513.469760	841656.740352	40.895143
3514.082340	841658.736594	40.900148
3514.372144	841638.107670	40.905152
3515.294220	841606.547402	40.910157
3516.200833	841553.091232	40.915162
3516.752991	841460.431621	40.920167
3516.830882	841358.777039	40.925172
3517.495253	841234.051826	40.930176
3517.813341	841099.479930	40.935181
3517.842248	840957.246234	40.940186
3518.707251	840791.068435	40.945191
3518.516621	840625.011402	40.950196
3518.508472	840434.237400	40.955200
3519.022946	840246.054584	40.960205
3519.446793	840044.514652	40.965210
3519.637092	839819.834183	40.970215
3519.814217	839598.806950	40.975220
3519.981979	839369.138136	40.980224
3520.204400	839119.594588	40.985229
3520.107504	838879.022799	40.990234
3520.482266	838619.773879	40.995239
3520.187056	838358.770575	41.000244
3520.014727	838116.718680	41.005248
3520.736974	837839.081805	41.010253
3520.143189	837577.803059	41.015258
3520.490600	837309.770137	41.020263
3520.158177	837035.688470	41.025268
3520.242350	836750.691119	41.030272
3520.153175	836462.878689	41.035277
3520.177895	836190.996234	41.040282
3520.192510	835899.529390	41.045287
3520.141388	835620.264326	41.050292
3520.027541	835345.049432	41.055296
3519.721383	835060.529691	41.060301
3519.789391	834763.827657	41.065306
3519.921368	834471.300418	41.070311
3519.716451	834193.512467	41.075316
3519.880515	833887.916599	41.080320
3520.093277	833598.217470	41.085325
3519.693466	833310.803795	41.090330
3519.876431	833010.486266	41.095335
3519.481050	832721.580605	41.100340
3519.672717	832419.817943	41.105344
3519.405042	832124.613014	41.110349
3519.138505	831827.684880	41.115354
3519.388305	831532.416623	41.120359
3519.189337	831247.906927	41.125364
3518.961434	830961.582027	41.130368
3519.068757	830666.297894	41.135373
3518.721157	830380.993084	41.140378
3518.801681	830091.745453	41.145383
3518.372371	829800.125935	41.150388
3518.343788	829511.505707	41.155392
3518.516503	829210.085841	41.160397
3517.801427	828938.265084	41.165402
3518.079669	828637.729886	41.170407
3517.896600	828367.948007	41.175412
3517.720936	828085.642234	41.180416
3517.566778	827810.212160	41.185421
3517.146145	827542.634761	41.190426
3517.464745	827261.825001	41.195431
3517.231541	826993.656635	41.200436
3516.981422	826718.831941	41.205440
3517.064051	826440.421170	41.210445
3516.591239	826173.969757	41.215450
3516.840725	825916.677560	41.220455
3516.357823	825651.819981	41.225460
3516.179141	825400.836216	41.230464
3516.315281	825136.247059	41.235469
3516.134523	824877.322641	41.240474
3516.061034	824623.162484	41.245479
3516.067734	824378.270484	41.250484
3515.918370	824116.132434	41.255488
3515.996942	823851.696807	41.260493
3515.812368	823606.709867	41.265498
3515.822473	823350.139385	41.270503
3515.808283	823099.725649	41.275508
3515.156990	822850.336698	41.280512
3515.141672	822602.936889	41.285517
3514.999342	822362.103470	41.290522
3515.148111	822119.794737	41.295527
3515.377680	821876.045175	41.300532
3514.837490	821635.397632	41.305536
3514.889491	821385.788761	41.310541
3514.532115	821145.337939	41.315546
3514.448671	820905.616112	41.320551
3514.512503	820681.126981	41.325556
3514.232312	820442.105832	41.330560
3514.481213	820219.283172	41.335565
3514.039049	819982.082635	41.340570
3514.086868	819751.203425	41.345575
3513.687640	819541.236846	41.350580
3513.245396	819311.010332	41.355584
3513.738267	819097.457153	41.360589
3513.711100	818877.473592	41.365594
3513.429506	818658.846146	41.370599
3513.303171	818447.919211	41.375604
3513.454028	818223.969224	41.380608
3513.648462	818010.626230	41.385613
3513.155583	817790.928323	41.390618
3513.215793	817568.341887	41.395623
3513.001393	817358.129331	41.400628
3512.802679	817145.019297	41.405632
3513.106640	816933.337310	41.410637
3512.694368	816726.515455	41.415642
3512.535678	816520.918373	41.420647
3512.069087	816318.792912	41.425652
3512.230640	816118.418435	41.430656
3512.414325	815918.426038	41.435661
3511.998164	815721.415393	41.440666
3512.236734	815518.806939	41.445671
3511.906535	815326.226446	41.450676
3511.736383	815133.760979	41.455680
3511.539205	814936.593316	41.460685
3511.539374	814767.154234	41.465690
3511.504298	814559.811735	41.470695
3511.378517	814388.816744	41.475700
3510.916034	814209.498064	41.480704
3511.363221	814020.474294	41.485709
3511.086869	813835.335727	41.490714
3510.853067	813658.119752	41.495719
3510.683683	813487.647856	41.500724
3510.573032	813314.272042	41.505728
3510.672971	813133.558580	41.510733
3510.405369	812966.469549	41.515738
3510.280533	812804.153469	41.520743
3510.773838	812634.922497	41.525748
3510.345484	812457.707065	41.530752
3510.497659	812282.301957	41.535757
3510.197985	812121.418984	41.540762
3510.206896	811954.063428	41.545767
3509.896515	811787.883168	41.550772
3510.179047	811623.658928	41.555776
3510.408986	811462.820058	41.560781
3509.988132	811306.200276	41.565786
3509.780662	811144.200981	41.570791
3509.758156	810994.123065	41.575796
3509.917595	810830.536883	41.580800
3509.890734	810663.253358	41.585805
3509.590596	810517.424732	41.590810
3509.308456	810362.916423	41.595815
3509.134032	810208.239844	41.600820
3509.570399	810049.293665	41.605824
3509.624013	809901.923394	41.610829
3509.245668	809758.835743	41.615834
3509.327582	809608.366966	41.620839
3509.521569	809451.456109	41.625844
3509.472292	809300.855116	41.630848
3509.617984	809136.250223	41.635853
3509.187132	808995.115651	41.640858
3509.326998	808844.228344	41.645863
3509.366459	808702.324043	41.650868
3509.030407	808558.419955	41.655872
3509.179604	808396.982699	41.660877
3508.822892	808261.555770	41.665882
3509.249842	808114.918674	41.670887
3508.797498	807970.482125	41.675892
3508.364870	807827.804048	41.680896
3508.742314	807686.068059	41.685901
3508.348619	807555.486452	41.690906
3508.473922	807419.816365	41.695911
3508.355752	807287.517423	41.700916
3508.221502	807151.541590	41.705920
3508.146418	807009.719045	41.710925
3507.781207	806894.024438	41.715930
3507.802160	806761.251150	41.720935
3507.733659	806639.129562	41.725940
3507.510799	806507.960485	41.730944
3507.658313	806394.722602	41.735949
3507.195283	806282.466001	41.740954
3507.353561	806156.179708	41.745959
3507.457667	806036.323524	41.750964
3507.222241	805933.977702	41.755968
3507.331781	805822.845143	41.760973
3507.425328	805706.270340	41.765978
3507.153583	805593.088282	41.770983
3507.508760	805485.734737	41.775988
3506.884363	805355.492445	41.780992
3507.220439	805242.842008	41.785997
3506.836636	805138.694283	41.791002
3507.025435	805025.181804	41.796007
3506.291730	804925.894563	41.801012
3506.532378	804825.121235	41.806016
3506.771182	804715.077457	41.811021
3506.732299	804617.534980	41.816026
3506.365672	804511.167912	41.821031
3506.583291	804412.354146	41.826036
3506.352900	804315.427483	41.831040
3506.463583	804212.018066	41.836045
3506.203997	804110.090481	41.841050
3506.330290	804009.765489	41.846055
3506.301480	803921.089324	41.851060
3506.190989	803811.726288	41.856064
3506.171649	803718.484280	41.861069
3506.150831	803639.220945	41.866074
3506.357726	803541.328435	41.871079
3506.176243	803444.970094	41.876084
3505.786766	803353.991502	41.881088
3506.179443	803247.528905	41.886093
3506.126161	803168.216451	41.891098
3506.048802	803075.171523	41.896103
3506.602495	802978.096903	41.901108
3505.913058	802889.025722	41.906112
3506.063129	802791.475337	41.911117
3505.867429	802704.920502	41.916122
3505.640279	802616.456471	41.921127
3505.948459	802523.242486	41.926132
3505.521898	802442.805759	41.931136
3505.586796	802351.052264	41.936141
3505.352068	802270.483812	41.941146
3505.725186	802181.915347	41.946151
3505.966423	802104.700895	41.951156
3505.581728	802013.654790	41.956160
3505.830478	801920.491538	41.961165
3505.491543	801839.346463	41.966170
3505.363684	801750.756871	41.971175
3505.153903	801681.953021	41.976180
3505.500098	801599.612847	41.981184
3505.573953	801519.720813	41.986189
3505.382135	801435.112107	41.991194
3505.386740	801351.892977	41.996199
3505.302355	801276.342161	42.001204
3505.025967	801201.509109	42.006208
3505.286097	801124.035272	42.011213
3505.251148	801049.553366	42.016218
3504.940757	800970.159917	42.021223
3505.134339	800888.523422	42.026228
3505.271091	800807.238830	42.031232
3505.184635	800731.240770	42.036237
3504.849904	800657.098461	42.041242
3505.136282	800579.957735	42.046247
3505.128452	800511.992323	42.051252
3504.859682	800445.835895	42.056256
3504.712892	800369.303994	42.061261
3504.770175	800308.000013	42.066266
3504.892019	800225.827718	42.071271
3505.211276	800148.431408	42.076276
3504.373052	800081.678238	42.081280
3504.759666	800008.195408	42.086285
3504.681046	799948.039413	42.091290
3504.604379	799881.011641	42.096295
3504.550119	799813.292431	42.101300
3504.390770	799758.399501	42.106304
3504.562290	799685.733958	42.111309
3504.361310	799624.466489	42.116314
3504.312662	799555.418684	42.121319
3504.521963	799488.438186	42.126324
3504.299431	799431.786172	42.131328
3504.764130	799354.111663	42.136333
3504.109018	799295.222941	42.141338
3504.549363	799241.405128	42.146343
3504.276719	799170.034427	42.151348
3503.977818	799122.472849	42.156352
3504.170880	799056.619792	42.161357
3504.065311	798996.214585	42.166362
3504.265798	798939.979734	42.171367
3504.091168	798887.045836	42.176372
3504.289960	798829.141475	42.181376
3504.324554	798768.956638	42.186381
3504.352155	798717.411634	42.191386
3504.141421	798652.013957	42.196391
3504.328140	798589.249997	42.201396
3504.143923	798528.019202	42.206400
3504.429414	798462.979805	42.211405
3504.571459	798407.584786	42.216410
3504.232524	798344.708855	42.221415
3504.318957	798284.560388	42.226420
3504.226414	798223.655445	42.231424
3503.832034	798154.797973	42.236429
3504.111625	798117.934107	42.241434
3504.146988	798044.193883	42.246439
3504.039064	797989.965817	42.251444
3503.634434	797936.964404	42.256448
3503.982976	797889.533225	42.261453
3503.788820	797845.971234	42.266458
3504.057775	797789.028536	42.271463
3503.964031	797723.750162	42.276468
3503.770769	797680.137896	42.281472
3504.100314	797621.711046	42.286477
3503.651213	797563.706529	42.291482
3503.520714	797497.057444	42.296487
3503.717308	797459.761924	42.301492
3503.591522	797419.229910	42.306496
3503.697547	797370.804153	42.311501
3503.392405	797327.159015	42.316506
3503.317083	797271.790791	42.321511
3503.569440	797234.779465	42.326516
3503.153346	797190.022519	42.331520
3503.351205	797146.244302	42.336525
3503.477585	797100.562775	42.341530
3503.555198	797054.103413	42.346535
3503.427698	797002.473101	42.351540
3503.525722	796961.606978	42.356544
3503.402335	796901.137472	42.361549
3503.475116	796867.541621	42.366554
3503.374139	796821.699325	42.371559
3503.276509	796776.003477	42.376564
3503.143075	796739.887781	42.381568
3503.260529	796688.165701	42.386573
3503.455680	796656.316303	42.391578
3503.558927	796618.295163	42.396583
3503.595971	796564.179459	42.401588
3503.324833	796522.487753	42.406592
3503.464815	796477.389141	42.411597
3503.001291	796437.005268	42.416602
3503.041298	796386.226660	42.421607
3503.366979	796350.278844	42.426612
3502.963035	796315.482192	42.431616
3503.482691	796267.668119	42.436621
3503.603807	796232.244429	42.441626
3503.606876	796188.197688	42.446631
3503.625154	796142.625927	42.451636
3503.690591	796099.943282	42.456640
3503.511115	796034.466847	42.461645
3503.746974	795995.389277	42.466650
3503.594889	795944.491793	42.471655
3503.785151	795894.617886	42.476660
3503.377017	795845.627893	42.481664
3503.405462	795809.431628	42.486669
3503.473665	795774.947373	42.491674
3503.352026	795735.632600	42.496679
3503.516304	795680.457864	42.501684
3503.258603	795641.557836	42.506688
3503.577455	795584.981867	42.511693
3503.475349	795537.265235	42.516698
3503.257046	795498.014161	42.521703
3503.416030	795454.771984	42.526708
3502.885044	795409.335040	42.531712
3503.460712	795358.166102	42.536717
3503.426658	795322.763380	42.541722
3502.886125	795285.921481	42.546727
3503.046092	795253.580409	42.551732
3503.122033	795211.283513	42.556736
3503.203499	795167.463005	42.561741
3503.467243	795135.693632	42.566746
3502.865716	795107.799125	42.571751
3502.780138	795053.299068	42.576756
3502.737050	795020.499248	42.581760
3503.034609	794987.053816	42.586765
3502.827909	794943.917841	42.591770
3502.316124	794917.972308	42.596775
3502.757345	794886.614593	42.601780
3502.345829	794849.601810	42.606784
3502.581482	794827.461905	42.611789
3502.240601	794801.782473	42.616794
3502.433382	794771.889469	42.621799
3502.715273	794742.620146	42.626804
3502.355246	794729.320374	42.631808
3502.613699	794685.025678	42.636813
3502.451863	794657.056952	42.641818
3502.336324	794635.563667	42.646823
3502.798601	794601.647238	42.651828
3502.365159	794574.705226	42.656832
3502.663397	794541.208448	42.661837
3502.949359	794522.399160	42.666842
3502.407526	794486.879401	42.671847
3502.595138	794458.950561	42.676852
3502.704305	794430.543366	42.681856
3502.695943	794390.121840	42.686861
3502.731179	794363.200051	42.691866
3502.741910	794337.215420	42.696871
3503.027143	794294.731188	42.701876
3502.525539	794261.512178	42.706880
3502.858270	794238.028256	42.711885
3502.720292	794206.517330	42.716890
3502.436707	794179.450881	42.721895
3502.854834	794149.174290	42.726900
3502.386798	794126.067485	42.731904
3502.741898	794092.166259	42.736909
3502.617192	794059.129805	42.741914
3502.511388	794024.518268	42.746919
3502.593207	793986.682889	42.751924
3502.356110	793959.607937	42.756928
3502.377323	793937.304078	42.761933
3502.301594	793907.009553	42.766938
3502.613035	793892.959033	42.771943
3502.951021	793860.533117	42.776948
3502.627319	793830.672072	42.781952
3502.491025	793797.587178	42.786957
3502.878992	793759.208944	42.791962
3502.415084	793730.500352	42.796967
3502.464286	793700.675574	42.801972
3502.578544	793676.292461	42.806977
3502.776387	793645.902631	42.811981
3502.668109	793618.952515	42.816986
3502.407837	793590.799275	42.821991
3502.550505	793554.670833	42.826996
3502.315999	793536.386748	42.832001
3502.811882	793510.564769	42.837005
3502.810531	793488.214084	42.842010
3502.603107	793470.956950	42.847015
3502.511747	793435.652416	42.852020
3502.395809	793404.330762	42.857025
3503.012572	793369.793485	42.862029
3502.758433	793334.957374	42.867034
3502.506320	793310.092977	42.872039
3502.576193	793277.315551	42.877044
3502.745798	793255.476338	42.882049
3502.764758	793212.783825	42.887053
3502.262919	793181.229994	42.892058
3502.150223	793163.907379	42.897063
3502.591750	793135.341971	42.902068
3502.082725	793114.350981	42.907073
3502.118825	793091.010356	42.912077
3502.377361	793067.780394	42.917082
3502.449372	793043.500305	42.922087
3502.347122	793023.719321	42.927092
3502.112682	792994.576919	42.932097
3501.740649	792971.106617	42.937101
3502.213356	792944.205604	42.942106
3501.912262	792923.130668	42.947111
3501.987606	792921.840964	42.952116
3501.891895	792899.651336	42.957121
3501.878777	792883.392426	42.962125
3502.050233	792868.527767	42.967130
3501.931527	792849.878934	42.972135
3501.946681	792828.604242	42.977140
3501.582190	792798.598154	42.982145
3501.622590	792777.220894	42.987149
3502.276696	792773.477693	42.992154
3502.050011	792749.540561	42.997159
3502.206099	792731.877843	43.002164
3501.951283	792733.934078	43.007169
3502.159116	792706.338867	43.012173
3502.154471	792692.239770	43.017178
3502.110035	792663.113830	43.022183
3501.997700	792647.853294	43.027188
3501.801048	792631.231002	43.032193
3502.059433	792597.142016	43.037197
3501.862496	792596.928815	43.042202
3502.051335	792584.418896	43.047207
3502.200090	792546.564770	43.052212
3502.141515	792549.620454	43.057217
3502.020144	792522.619174	43.062221
3501.909178	792499.742987	43.067226
3502.121000	792491.208634	43.072231
3502.085403	792460.753896	43.077236
3502.066017	792442.578928	43.082241
3501.967869	792418.865152	43.087245
3502.153489	792403.407619	43.092250
3501.951207	792384.230885	43.097255
3502.271955	792356.075272	43.102260
3502.501924	792339.283761	43.107265
3502.635300	792309.734028	43.112269
3502.568166	792281.740271	43.117274
3502.151684	792258.127522	43.122279
3502.467741	792233.165741	43.127284
3502.411952	792222.218559	43.132289
3502.373210	792192.942348	43.137293
3502.276725	792167.360439	43.142298
3502.592990	792152.519557	43.147303
3502.558752	792113.808876	43.152308
3502.131749	792082.336061	43.157313
3502.143853	792059.487309	43.162317
3502.420571	792044.898381	43.167322
3502.245577	792022.522524	43.172327
3502.475527	791980.328274	43.177332
3502.313741	791967.285417	43.182337
3502.412202	791947.271824	43.187341
3502.311850	791934.071385	43.192346
3501.554022	791912.822991	43.197351
3501.858060	791880.639257	43.202356
3501.618918	791884.707652	43.207361
3501.814051	791865.267513	43.212365
3501.568354	791841.772641	43.217370
3501.596558	791832.678128	43.222375
3502.021929	791823.370781	43.227380
3501.444147	791802.878551	43.232385
3501.534752	791779.770291	43.237389
3501.602694	791778.285061	43.242394
3501.675730	791768.102113	43.247399
3501.932341	791758.871614	43.252404
3501.764293	791745.534569	43.257409
3501.895959	791733.573052	43.262413
3501.629306	791722.266746	43.267418
3502.145015	791694.764286	43.272423
3502.094928	791684.306685	43.277428
3502.074790	791663.034300	43.282433
3502.094667	791628.734259	43.287437
3502.131928	791624.502439	43.292442
3502.035663	791601.522650	43.297447
3502.391403	791577.731292	43.302452
3502.055842	791568.450675	43.307457
3501.936464	791548.864927	43.312461
3502.210482	791526.954044	43.317466
3502.146965	791502.936673	43.322471
3502.143033	791470.801805	43.327476
3501.620927	791464.745683	43.332481
3501.688048	791443.310853	43.337485
3501.756208	791433.668738	43.342490
3501.686278	791423.607118	43.347495
3501.776088	791400.399478	43.352500
3501.672638	791390.589021	43.357505
3501.875041	791386.870371	43.362509
3501.535932	791369.924611	43.367514
3501.570440	791354.538818	43.372519
3501.765733	791339.421336	43.377524
3501.837908	791336.412041	43.382529
3501.978783	791315.062952	43.387533
3502.057158	791287.336120	43.392538
3501.560485	791290.022263	43.397543
3502.115407	791258.531456	43.402548
3502.018087	791243.019720	43.407553
3501.632005	791237.579796	43.412557
3502.101497	791206.741633	43.417562
3501.839378	791194.106986	43.422567
3501.860788	791183.243757	43.427572
3502.138623	791169.242514	43.432577
3501.982106	791161.258625	43.437581
3501.904196	791146.333149	43.442586
3501.833313	791121.087215	43.447591
3501.944108	791100.970920	43.452596
3501.760070	791094.907932	43.457601
3502.273373	791076.592575	43.462605
3502.035183	791054.764602	43.467610
3501.718516	791043.268887	43.472615
3501.869702	791014.447916	43.477620
3501.989833	791019.636990	43.482625
3502.167899	790994.103897	43.487629
3502.041541	790973.682322	43.492634
3502.260991	790962.393012	43.497639
3501.844154	790936.711998	43.502644
3502.103383	790930.035308	43.507649
3501.946680	790902.443974	43.512653
3502.311159	790882.039570	43.517658
3502.083895	790866.155283	43.522663
3502.181301	790836.654472	43.527668
3502.047062	790821.000469	43.532673
3502.139487	790801.328624	43.537677
3502.119524	790783.051207	43.542682
3502.011072	790769.407654	43.547687
3502.130501	790741.426217	43.552692
3501.840345	790720.736041	43.557697
3501.867194	790694.784499	43.562701
3502.287469	790690.587319	43.567706
3502.192408	790675.565392	43.572711
3502.278458	790650.881644	43.577716
3501.848486	790637.929651	43.582721
3501.577933	790601.559337	43.587725
3501.388632	790606.406538	43.592730
3501.452865	790600.105659	43.597735
3501.869071	790582.837029	43.602740
3501.921396	790565.235147	43.607745
3501.605633	790550.740741	43.612749
3501.982226	790540.997466	43.617754
3501.885138	790520.569765	43.622759
3502.112195	790502.644086	43.627764
3501.837185	790501.067647	43.632769
3501.788826	790482.450127	43.637773
3501.941863	790457.017513	43.642778
3501.862439	790458.406633	43.647783
3501.783620	790425.296482	43.652788
3501.733253	790425.697938	43.657793
3501.659298	790409.345076	43.662797
3501.712966	790402.750896	43.667802
3501.793023	790387.797804	43.672807
3501.549638	790369.605266	43.677812
3501.623018	790369.986343	43.682817
3501.387300	790353.217694	43.687821
3502.037056	790318.561841	43.692826
3501.483244	790321.749200	43.697831
3501.905804	790316.371948	43.702836
3501.692258	790287.853829	43.707841
3501.856303	790269.544780	43.712845
3501.780115	790271.572293	43.717850
3501.729125	790265.093515	43.722855
3501.815049	790236.034408	43.727860
3501.639870	790239.700038	43.732865
3501.616363	790229.727368	43.737869
3501.733246	790210.492169	43.742874
3501.680846	790194.086114	43.747879
3501.927279	790174.190582	43.752884
3501.556904	790180.493131	43.757889
3501.406275	790152.504710	43.762893
3501.613835	790127.602544	43.767898
3501.296236	790128.932667	43.772903
3501.455324	790125.957691	43.777908
3501.473005	790126.937710	43.782913
3501.431525	790121.046990	43.787917
3501.629471	790101.257533	43.792922
3501.130642	790079.174605	43.797927
3501.404176	790060.601251	43.802932
3501.778207	790064.520536	43.807937
3501.731287	790063.938509	43.812941
3501.779769	790043.682044	43.817946
3501.234453	790038.562300	43.822951
3501.589293	790033.736606	43.827956
3501.847346	790034.382165	43.832961
3501.667020	790012.590596	43.837965
3501.884371	789988.177800	43.842970
3501.545623	789984.056084	43.847975
3501.660527	789974.994057	43.852980
3501.797620	789955.459954	43.857985
3501.712538	789936.404723	43.862989
3501.793416	789930.641133	43.867994
3501.907859	789927.820872	43.872999
3502.043537	789896.737127	43.878004
3501.603486	789880.148459	43.883009
3501.538053	789874.359775	43.888013
3501.742266	789856.485380	43.893018
3501.976595	789846.125664	43.898023
3501.828116	789838.679589	43.903028
3501.855160	789819.605576	43.908033
3501.921663	789803.670519	43.913037
3501.867839	789788.443327	43.918042
3501.361116	789788.428500	43.923047
3501.893925	789760.768301	43.928052
3501.700852	789760.898407	43.933057
3501.591203	789741.895849	43.938061
3501.983725	789731.165867	43.943066
3501.961078	789714.999550	43.948071
3501.999247	789696.021671	43.953076
3501.655438	789693.375096	43.958081
3501.817279	789681.011959	43.963085
3501.432680	789667.460921	43.968090
3501.773267	789680.970071	43.973095
3501.830117	789658.794305	43.978100
3501.714153	789629.471075	43.983105
3502.092688	789624.936103	43.988109
3502.049217	789593.044994	43.993114
3502.037849	789585.870969	43.998119
3502.134315	789558.773360	44.003124
3502.086697	789540.988802	44.008129
3501.764289	789522.217303	44.013133
3501.756655	789511.995258	44.018138
3501.807268	789488.836978	44.023143
3501.764503	789480.979909	44.028148
3501.416964	789480.398199	44.033153
3501.722242	789472.090587	44.038157
3502.157164	789440.808109	44.043162
3501.982431	789429.777901	44.048167
3501.902608	789411.555965	44.053172
3502.142269	789396.377895	44.058177
3502.089630	789394.027306	44.063181
3501.999277	789345.136412	44.068186
3501.769525	789350.630099	44.073191
3501.940615	789340.230914	44.078196
3502.071453	789302.460731	44.083201
3502.214472	789297.423674	44.088205
3502.360219	789267.711780	44.093210
3502.041943	789255.721901	44.098215
3502.297054	789234.740965	44.103220
3502.203549	789212.146201	44.108225
3502.094855	789187.784365	44.113229
3502.214645	789155.667793	44.118234
3501.873420	789155.625697	44.123239
3501.938245	789126.909606	44.128244
3502.064828	789103.737560	44.133249
3501.844801	789093.844818	44.138253
3502.098078	789064.556747	44.143258
3501.831452	789056.146238	44.148263
3502.023891	789039.156498	44.153268
3501.762153	789023.666992	44.158273
3501.711006	789003.079897	44.163277
3501.416936	788996.148459	44.168282
3501.682043	788978.605910	44.173287
3501.805962	788950.665842	44.178292
3501.647762	788961.210947	44.183297
3501.474967	788959.961401	44.188301
3501.704374	788938.148202	44.193306
3501.541018	788929.769688	44.198311
3501.526219	788922.251477	44.203316
3501.402589	788914.652875	44.208321
3501.210438	788919.255915	44.213325
3501.706368	788905.410919	44.218330
3501.482960	788902.596748	44.223335
3501.421725	788874.146175	44.228340
3501.565117	788869.846079	44.233345
3501.283311	788867.483908	44.238349
3501.607037	788860.892973	44.243354
3501.088920	788848.148840	44.248359
3501.527613	788831.363820	44.253364
3501.569459	788827.031269	44.258369
3501.563458	788827.376351	44.263373
3501.774644	788819.476722	44.268378
3501.487293	788804.974064	44.273383
3501.806371	788785.210155	44.278388
3501.698970	788786.604208	44.283393
3501.505944	788779.164358	44.288397
3501.543777	788768.196422	44.293402
3501.326528	788758.007821	44.298407
3501.428689	788727.170270	44.303412
3501.328064	788732.643161	44.308417
3501.159794	788723.232937	44.313421
3501.612936	788723.354929	44.318426
3501.574343	788726.458119	44.323431
3501.418558	788703.675374	44.328436
3501.554650	788694.460760	44.333441
3501.454164	788680.811881	44.338445
3501.620777	788673.607621	44.343450
3501.466563	788682.677790	44.348455
3501.483673	788658.440889	44.353460
3501.893604	788644.806181	44.358465
3501.297781	788639.595419	44.363469
3501.480760	788629.439023	44.368474
3501.660387	788637.077876	44.373479
3501.365300	788609.844524	44.378484
3501.496871	788594.436768	44.383489
3501.742716	788583.581756	44.388493
3501.981880	788581.871031	44.393498
3501.701807	788579.164378	44.398503
3501.408416	788550.013395	44.403508
3501.683138	788543.331925	44.408513
3501.403896	788543.279612	44.413517
3501.659217	788530.456668	44.418522
3501.481002	788515.247240	44.423527
3501.502789	788495.334868	44.428532
3501.566011	788498.716332	44.433537
3501.349335	788494.180374	44.438541
3501.813188	788486.877809	44.443546
3501.598777	788471.084356	44.448551
3501.502672	788450.798016	44.453556
3501.784488	788443.476233	44.458561
3501.330921	788438.241890	44.463565
3501.857056	788421.343189	44.468570
3501.389865	788410.015464	44.473575
3501.211076	788402.523716	44.478580
3501.561135	788401.679531	44.483585
3501.510524	788407.341066	44.488589
3501.595153	788393.611987	44.493594
3501.725197	788365.521143	44.498599
3501.763999	788357.649399	44.503604
3501.750597	788354.210515	44.508609
3501.483218	788346.290873	44.513613
3501.829431	788311.822749	44.518618
3501.581010	788313.977503	44.523623
3501.459605	788310.507229	44.528628
3501.576068	788301.688613	44.533633
3501.583025	788291.855684	44.538637
3501.456322	788273.589397	44.543642
3501.414214	788256.587270	44.548647
3501.701844	788254.475211	44.553652
3501.381880	788262.000120	44.558657
3501.465373	788243.797453	44.563661
3501.298069	788232.272569	44.568666
3501.401140	788216.032982	44.573671
3501.193020	788211.249636	44.578676
3501.607021	788206.118016	44.583681
3501.514202	788213.458083	44.588685
3501.503265	788200.088489	44.593690
3501.357249	788190.870534	44.598695
3501.272816	788193.981506	44.603700
3501.245445	788178.451554	44.608705
3501.293015	788189.897939	44.613709
3501.538710	788191.332266	44.618714
3501.469252	788182.839085	44.623719
3501.479209	788176.938281	44.628724
3501.700025	788150.208111	44.633729
3501.452188	788151.477938	44.638733
3501.660661	788137.580488	44.643738
3501.406143	788141.801019	44.648743
3501.791174	788128.071109	44.653748
3501.327920	788095.455875	44.658753
3501.559717	788098.711442	44.663757
3501.803145	788086.627067	44.668762
3501.379739	788084.927039	44.673767
3501.650108	788061.039677	44.678772
3501.572854	788047.729881	44.683777
3501.660535	788041.767003	44.688781
3501.734358	788025.826765	44.693786
3501.275522	788016.512627	44.698791
3501.227566	787997.937698	44.703796
3501.327862	787990.792835	44.708801
3501.343135	788003.572187	44.713805
3501.136516	787990.971847	44.718810
3501.442646	788000.606150	44.723815
3501.789556	787992.142482	44.728820
3501.675539	787974.217465	44.733825
3501.566214	787959.290469	44.738829
3501.617298	787950.088898	44.743834
3501.425005	787942.844697	44.748839
3501.424874	787935.273868	44.753844
3501.523311	787917.903653	44.758849
3501.626704	787920.737998	44.763853
3501.783659	787899.474337	44.768858
3501.107931	787894.374505	44.773863
3501.424794	787899.484298	44.778868
3501.343699	787886.125672	44.783873
3501.143163	787872.786695	44.788877
3501.568380	787857.181496	44.793882
3501.257040	787857.183622	44.798887
3501.196628	787840.527651	44.803892
3501.281058	787844.053419	44.808897
3501.210354	787841.361158	44.813901
3501.494332	787849.671937	44.818906
3501.272317	787867.898438	44.823911
3501.567764	787842.531357	44.828916
3501.440655	787823.575715	44.833921
3501.364750	787821.916709	44.838925
3501.379404	787820.636083	44.843930
3501.316208	787818.630847	44.848935
3501.353888	787808.546381	44.853940
3501.557929	787797.451251	44.858945
3501.442615	787777.903596	44.863949
3501.534603	787758.567555	44.868954
3501.630612	787758.895886	44.873959
3501.500416	787761.572120	44.878964
3501.322923	787759.290717	44.883969
3501.264835	787739.438555	44.888973
3501.572044	787717.117184	44.893978
3501.574186	787714.904505	44.898983
3501.539260	787712.452116	44.903988
3501.612865	787709.883524	44.908993
3501.326040	787699.803192	44.913997
3501.276706	787678.425363	44.919002
3501.144658	787668.909452	44.924007
3501.336273	787675.662424	44.929012
3501.382145	787655.448762	44.934017
3501.366762	787658.597756	44.939021
3501.627962	787663.274418	44.944026
3501.384589	787665.281043	44.949031
3501.425437	787644.527381	44.954036
3502.126609	787625.533110	44.959041
3501.764353	787630.951611	44.964045
3502.094067	787610.396088	44.969050
3501.893711	787594.500049	44.974055
3501.558523	787582.706785	44.979060
3501.745096	787572.646625	44.984065
3501.768049	787551.944806	44.989069
3501.463396	787532.034352	44.994074
3501.741459	787542.460526	44.999079
3501.715577	787535.434320	45.004084
3501.971212	787500.288904	45.009089
3501.769077	787494.914116	45.014093
3502.198597	787474.095940	45.019098
3502.085267	787456.759486	45.024103
3502.049620	787451.160582	45.029108
3501.933926	787426.646385	45.034113
3501.678318	787403.826762	45.039117
3502.041142	787401.898732	45.044122
3501.914472	787380.975238	45.049127
3501.738552	787356.421554	45.054132
3501.724486	787349.098226	45.059137
3501.629335	787343.017384	45.064141
3501.854532	787313.235102	45.069146
3501.897090	787317.603845	45.074151
3501.590561	787304.772920	45.079156
3501.511850	787283.890407	45.084161
3501.416385	787275.351263	45.089165
3501.530608	787261.123474	45.094170
3501.180533	787263.737777	45.099175
3501.033380	787259.828736	45.104180
3501.435157	787266.694978	45.109185
3501.259052	787267.854810	45.114189
3501.307362	787251.769550	45.119194
3501.362292	787235.437332	45.124199
3501.159241	787230.799988	45.129204
3501.263978	787221.490309	45.134209
3501.049876	787213.708128	45.139213
3501.194175	787205.424406	45.144218
3501.266336	787212.541658	45.149223
3501.335155	787212.333663	45.154228
3501.111025	787213.550580	45.159233
3500.762611	787215.279633	45.164237
3500.995692	787216.912904	45.169242
3500.649786	787224.295672	45.174247
3501.082709	787232.877638	45.179252
3501.347230	787219.805001	45.184257
3501.115756	787222.694782	45.189261
3501.529642	787222.626616	45.194266
3501.503283	787207.192717	45.199271
3501.489795	787194.755823	45.204276
3501.531275	787184.129019	45.209281
3501.311187	787174.331949	45.214285
3501.081914	787172.255553	45.219290
3501.445669	787174.457310	45.224295
3501.451852	787164.819624	45.229300
3501.567397	787160.326424	45.234305
3501.159388	787141.169404	45.239309
3501.327651	787123.638257	45.244314
3501.518448	787133.587734	45.249319
3501.498880	787120.905879	45.254324
3501.416888	787118.362704	45.259329
3501.243276	787126.503866	45.264333
3501.673872	787114.485356	45.269338
3501.637391	787086.023574	45.274343
3501.567759	787090.509270	45.279348
3501.478284	787083.001422	45.284353
3501.584497	787082.541427	45.289357
3501.609475	787058.445301	45.294362
3501.669339	787049.634465	45.299367
3501.681056	787032.915562	45.304372
3501.746949	787035.510599	45.309377
3501.597943	787016.802259	45.314381
3501.691621	786997.513050	45.319386
3501.496485	787000.446103	45.324391
3501.626032	786985.821900	45.329396
3501.947541	786973.132770	45.334401
3501.531929	786964.842660	45.339405
3501.545453	786954.515128	45.344410
3501.664840	786943.875134	45.349415
3501.617133	786937.638627	45.354420
3501.705713	786914.662411	45.359425
3501.638854	786904.839732	45.364429
3501.547729	786895.266879	45.369434
3501.427450	786899.220183	45.374439
3501.445744	786866.667514	45.379444
3501.687577	786849.172747	45.384449
3501.399138	786854.579672	45.389453
3501.537860	786847.574846	45.394458
3501.848069	786850.375553	45.399463
3501.568479	786824.116203	45.404468
3501.569191	786818.854999	45.409473
3501.583290	786819.393543	45.414477
3501.589898	786814.328040	45.419482
3501.205744	786798.804686	45.424487
3501.466784	786775.357094	45.429492
3501.336227	786764.561325	45.434497
3501.532287	786764.578207	45.439501
3501.654730	786757.133449	45.444506
3501.318585	786751.681832	45.449511
3501.267801	786745.544004	45.454516
3501.598705	786732.312036	45.459521
3501.573448	786731.185299	45.464525
3501.733554	786720.144908	45.469530
3501.533438	786728.340057	45.474535
3501.425946	786725.309244	45.479540
3501.800035	786692.943030	45.484545
3501.598892	786693.566207	45.489549
3501.423902	786680.319131	45.494554
3501.748811	786670.628280	45.499559
3501.343611	786660.910166	45.504564
3501.833315	786639.538783	45.509569
3501.757787	786643.829048	45.514573
3501.445641	786631.686221	45.519578
3501.618041	786618.971856	45.524583
3501.519870	786606.056182	45.529588
3501.476999	786592.492158	45.534593
3501.234175	786600.841999	45.539597
3501.856865	786583.382193	45.544602
3501.440349	786569.289620	45.549607
3501.306956	786569.311598	45.554612
3501.754946	786555.715823	45.559617
3501.379435	786551.548981	45.564621
3501.628147	786548.410250	45.569626
3501.496048	786538.646985	45.574631
3501.382330	786513.096736	45.579636
3501.637450	786502.532073	45.584641
3501.443520	786499.072860	45.589645
3501.226216	786493.208100	45.594650
3501.416289	786488.603861	45.599655
3501.264259	786491.431677	45.604660
3501.493104	786461.989454	45.609665
3501.185204	786460.368342	45.614669
3501.368076	786447.111060	45.619674
3501.110826	786451.234686	45.624679
3500.975115	786458.681959	45.629684
3501.460726	786453.291445	45.634689
3501.371015	786442.881836	45.639693
3501.252201	786431.247711	45.644698
3501.588007	786440.584208	45.649703
3501.204420	786414.094623	45.654708
3501.450363	786396.893107	45.659713
3501.194881	786397.033539	45.664717
3500.999173	786406.703488	45.669722
3501.197077	786408.490258	45.674727
3501.030035	786402.764660	45.679732
3501.494776	786399.000218	45.684737
3501.405250	786400.047582	45.689741
3501.652056	786400.449484	45.694746
3501.453109	786379.485790	45.699751
3501.446477	786360.899799	45.704756
3501.686225	786339.716213	45.709761
3501.407955	786360.365261	45.714765
3501.269970	786362.453230	45.719770
3501.289661	786348.976784	45.724775
3501.072850	786337.801200	45.729780
3501.250296	786313.529935	45.734785
3501.147669	786312.907602	45.739789
3501.480986	786308.082963	45.744794
3501.546309	786301.433903	45.749799
3501.165886	786305.037001	45.754804
3501.587018	786303.443288	45.759809
3501.367080	786306.134844	45.764813
3501.606453	786275.411632	45.769818
3501.295941	786204.063457	45.774823
3501.287822	786078.179956	45.779828
3501.192772	785904.362717	45.784833
3500.899616	785671.414221	45.789837
3500.858048	785378.418592	45.794842
3500.572776	785038.974946	45.799847
3500.207272	784648.623219	45.804852
3500.247645	784192.027075	45.809857
3499.816609	783678.615478	45.814861
3499.878995	783105.856046	45.819866
3499.324634	782484.249326	45.824871
3498.716849	781802.422392	45.829876
3498.312305	781060.119198	45.834881
3497.967996	780271.223150	45.839885
3497.624614	779419.634197	45.844890
3496.998033	778518.865144	45.849895
3496.031063	777555.811637	45.854900
3496.019905	776526.247413	45.859905
3495.256958	775441.555760	45.864909
3494.458710	774307.997567	45.869914
3493.997568	773105.439739	45.874919
3493.363863	771856.597421	45.879924
3492.661042	770551.772042	45.884929
3491.919980	769181.022752	45.889933
3491.028149	767744.677523	45.894938
3490.228093	766256.021754	45.899943
3489.370226	764714.803340	45.904948
3488.577673	763104.643225	45.909953
3487.963545	761451.382862	45.914957
3486.799626	759732.414427	45.919962
3486.099434	757953.056399	45.924967
3484.185814	756124.505483	45.929972
3483.422329	754222.386952	45.934977
3482.484570	752282.828474	45.939981
3481.295857	750286.744271	45.944986
3480.066861	748235.046969	45.949991
3478.730191	746126.519987	45.954996
3477.851526	743961.670050	45.960001
3476.582881	741756.372770	45.965005
3474.962887	739486.346869	45.970010
3474.153751	737166.097980	45.975015
3472.362037	734798.505726	45.980020
3471.292795	732362.699709	45.985025
3469.625162	729882.222172	45.990029
3468.112672	727345.367006	45.995034
3466.718906	724766.566824	46.000039
3465.087349	722131.615676	46.005044
3463.711504	719445.641928	46.010049
3462.067392	716724.615379	46.015053
3460.254654	713946.802382	46.020058
3458.896700	711111.107482	46.025063
3457.187496	708237.230555	46.030068
3455.673062	705303.140537	46.035073
3453.807526	702333.773084	46.040077
3452.005293	699301.190486	46.045082
3450.506981	696224.841356	46.050087
3448.314165	693113.659230	46.055092
3446.683952	689928.141923	46.060097
3444.613404	686714.238780	46.065101
3442.953291	683437.075679	46.070106
3441.077876	680135.160954	46.075111
3438.911058	676786.162787	46.080116
3437.150060	673383.644321	46.085121
3434.837364	669940.086050	46.090125
3432.798409	666446.986680	46.095130
3430.854596	662905.332055	46.100135
3428.733868	659332.802165	46.105140
3426.960509	655703.715662	46.110145
3424.640969	652038.857883	46.115149
3422.266798	648325.175855	46.120154
3420.132152	644568.482280	46.125159
3418.015557	640784.438532	46.130164
3416.031831	636938.982283	46.135169
3413.349610	633066.189652	46.140173
3410.833429	629152.933815	46.145178
3408.614031	625202.071110	46.150183
3406.017107	621209.929831	46.155188
3404.163715	617164.766642	46.160193
3401.560719	613078.322844	46.165197
3399.162519	608955.532145	46.170202
3397.177715	604801.910902	46.175207
3394.691283	600603.789003	46.180212
3392.286345	596358.932792	46.185217
3389.762817	592083.272993	46.190221
3386.928862	587774.416855	46.195226
3384.530989	583417.093306	46.200231
3382.083771	579036.250695	46.205236
3379.199601	574598.239284	46.210241
3376.530625	570137.896568	46.215245
3373.555902	565637.686237	46.220250
3370.755392	561110.809514	46.225255
3367.891316	556554.834219	46.230260
3365.516178	551964.775954	46.235265
3362.671441	547332.313624	46.240269
3359.695120	542682.190028	46.245274
3356.688780	537996.285167	46.250279
3353.724927	533274.125032	46.255284
3351.042039	528505.767806	46.260289
3348.274524	523742.365349	46.265293
3345.272252	518925.779842	46.270298
3342.283801	514090.665814	46.275303
3339.252992	509217.988357	46.280308
3336.418445	504326.513703	46.285313
3333.460238	499404.472901	46.290317
3330.347875	494441.300940	46.295322
3327.575575	489454.270581	46.300327
3324.326602	484441.452553	46.305332
3321.004011	479400.259343	46.310337
3317.870341	474342.103996	46.315341
3314.801973	469245.038531	46.320346
3311.731139	464139.989648	46.325351
3308.513790	459009.977260	46.330356
3305.418479	453836.111253	46.335361
3302.286039	448657.014014	46.340365
3298.969627	443441.747226	46.345370
3295.841110	438210.859514	46.350375
3292.495845	432964.696659	46.355380
3289.716964	427683.257276	46.360385
3286.021105	422378.426416	46.365389
3282.510682	417065.127344	46.370394
3279.342845	411720.712840	46.375399
3275.878786	406366.695692	46.380404
3272.557081	400998.209192	46.385409
3269.001024	395589.197917	46.390413
3265.424196	390177.741755	46.395418
3262.571686	384743.877812	46.400423
3258.656681	379305.090272	46.405428
3255.177325	373836.708071	46.410433
3251.602165	368363.158286	46.415437
3248.168329	362861.548322	46.420442
3244.361141	357356.515250	46.425447
3240.818789	351849.749238	46.430452
3237.502385	346308.931072	46.435457
3233.757808	340772.217505	46.440461
3230.148270	335201.026540	46.445466
3226.661587	329628.430056	46.450471
3222.860113	324061.669854	46.455476
3219.146014	318471.039981	46.460481
3215.374322	312881.475266	46.465485
3211.338063	307289.182766	46.470490
3207.726405	301661.167689	46.475495
3203.908409	296051.580843	46.480500
3200.043615	290430.953141	46.485505
3196.209099	284825.671533	46.490509
3192.301695	279206.154084	46.495514
3188.730217	273581.314707	46.500519
3184.777204	267941.942531	46.505524
3180.664133	262295.990356	46.510529
3177.123549	256679.902784	46.515533
3172.922672	251032.268090	46.520538
3169.230520	245393.431976	46.525543
3165.139579	239760.327609	46.530548
3161.260548	234104.044459	46.535553
3156.860628	228468.015082	46.540557
3152.723177	222833.894119	46.545562
3149.082231	217208.408606	46.550567
3144.512272	211557.514241	46.555572
3140.756631	205876.262834	46.560577
3136.907633	200275.517503	46.565581
3132.797086	194653.026676	46.570586
3128.615576	189042.405579	46.575591
3124.515076	183448.199319	46.580596
3120.409096	177852.545360	46.585601
3115.966447	172262.360934	46.590605
3111.599134	166692.171599	46.595610
3107.470065	161138.653356	46.600615
3103.237085	155587.044706	46.605620
3098.650870	150051.491343	46.610625
3094.167828	144526.537160	46.615629
3090.012496	139022.897707	46.620634
3085.486675	133519.469426	46.625639
3080.482031	128054.839048	46.630644
3076.573292	122604.476146	46.635649
3071.908729	117169.518697	46.640653
3066.919108	111761.357067	46.645658
3062.844745	106367.507182	46.650663
3057.894291	101017.124525	46.655668
3053.155991	95671.857567	46.660673
3047.945596	90360.449320	46.665677
3042.879593	85090.793507	46.670682
3037.951951	79848.307700	46.675687
3032.229400	74662.949890	46.680692
3026.434103	69517.906532	46.685697
3019.349244	64441.261227	46.690701
3008.767253	59519.152729	46.695706
2993.865221	54839.516072	46.700711
2978.473113	50321.793193	46.705716
2963.606981	46013.205865	46.710721
2949.394205	41925.676579	46.715725
2935.622656	38064.530001	46.720730
2922.361474	34434.378344	46.725735
2909.434478	31071.393938	46.730740
2897.684028	27919.357935	46.735745
2886.181348	25002.556696	46.740749
2874.860365	22319.353294	46.745754
2865.012881	19829.665937	46.750759
2855.398168	17547.278647	46.755764
2846.211001	15451.000716	46.760769
2835.877481	13566.533482	46.765773
2823.664806	11905.853331	46.770778
2811.733904	10481.813088	46.775783
2799.335058	9251.641730	46.780788
2788.056706	8198.588218	46.785793
2778.108522	7337.075392	46.790797
2769.796371	6640.559873	46.795802
2762.554221	6060.237853	46.800807
2756.465864	5603.858229	46.805812
2751.715898	5251.804137	46.810817
2747.922072	4959.627217	46.815821
2744.777857	4728.157060	46.820826
2742.290997	4527.548313	46.825831
2740.053143	4350.375277	46.830836
2738.033266	4201.527567	46.835841
2736.098379	4066.861974	46.840845
2733.717416	3929.152697	46.845850
2732.436581	3774.735167	46.850855
2730.558271	3637.111780	46.855860
2728.020774	3482.611042	46.860865
2726.234120	3331.283943	46.865869
2723.991915	3165.232446	46.870874
2722.137203	2991.185578	46.875879
2719.857221	2806.264824	46.880884
2717.223279	2605.679011	46.885889
2714.713358	2396.982930	46.890893
2711.966760	2193.547648	46.895898
2709.263148	1968.198681	46.900903
2706.316455	1744.556438	46.905908
2703.172588	1516.229861	46.910913
2700.552903	1287.957187	46.915917
2697.108091	1065.982399	46.920922
2693.790495	823.142030	46.925927
2690.002492	589.746263	46.930932
2686.062218	367.005673	46.935937
2682.105402	153.678293	46.940941
2672.197565	124.759385	46.945946
2659.629012	203.040072	46.950951
2654.395761	209.294164	46.955956
2652.217316	207.676701	46.960961
2650.750157	206.037960	46.965965
2649.106321	206.726030	46.970970
2647.058219	206.243170	46.975975
2644.302087	197.635827	46.980980
2641.542942	203.286359	46.985985
2638.049471	196.208362	46.990989
2634.052980	208.384119	46.995994
2630.824910	197.390475	47.000999
2627.485666	192.996047	47.006004
2624.294048	203.658161	47.011009
2621.468887	190.338006	47.016013
2617.893328	207.619936	47.021018
2614.526492	203.626376	47.026023
2610.738613	189.680421	47.031028
2607.312676	199.529446	47.036033
2604.462042	188.539396	47.041037
2600.898241	206.458112	47.046042
2597.702623	185.110759	47.051047
2594.114454	192.731478	47.056052
2590.691803	191.347402	47.061057
2587.179188	190.928645	47.066061
2583.771539	196.455060	47.071066
2580.938376	178.348810	47.076071
2577.074901	193.571441	47.081076
2573.678408	189.148199	47.086081
2570.911929	188.191757	47.091085
2567.088258	190.217083	47.096090
2563.715312	190.356114	47.101095
2560.094878	186.976920	47.106100
2556.817796	189.770164	47.111105
2553.166419	177.256974	47.116109
2549.329863	179.617703	47.121114
2545.710979	178.439054	47.126119
2542.361648	189.447139	47.131124
2539.247817	189.033782	47.136129
2535.939739	186.688940	47.141133
2532.265382	183.690597	47.146138
2529.034107	172.131942	47.151143
2525.651995	177.736641	47.156148
2522.404729	185.080175	47.161153
2519.480317	181.610405	47.166157
2515.963593	175.251695	47.171162
2512.551241	165.810146	47.176167
2508.368170	169.390136	47.181172
2504.330375	181.660441	47.186177
2501.395986	169.839448	47.191181
2497.971838	186.843559	47.196186
2494.648738	177.801170	47.201191
2491.138752	178.764535	47.206196
2487.578800	173.134069	47.211201
2484.491113	173.915132	47.216205
2480.827000	177.309325	47.221210
2477.672854	175.454425	47.226215
2473.821866	195.405640	47.231220
2470.011416	175.319310	47.236225
2466.602289	172.578868	47.241229
2463.273503	182.704534	47.246234
2460.366704	164.587228	47.251239
2456.504599	176.130268	47.256244
2452.823230	178.046347	47.261249
2449.609487	174.275066	47.266253
2445.781584	179.407724	47.271258
2442.691597	170.010230	47.276263
2439.606563	170.203063	47.281268
2435.736833	175.641953	47.286273
2432.233776	175.995574	47.291277
2428.403542	186.252189	47.296282
2425.346550	175.560080	47.301287
2421.689330	174.802576	47.306292
2417.933025	168.677492	47.311297
2414.658705	171.195372	47.316301
2411.096304	181.074257	47.321306
2407.673014	173.828051	47.326311
2404.289509	176.757393	47.331316
2400.795777	172.369417	47.336321
2397.576249	171.333055	47.341325
2394.189822	171.209584	47.346330
2390.597788	169.763460	47.351335
2387.150407	176.559430	47.356340
2383.248912	165.105664	47.361345
2380.056812	161.765639	47.366349
2376.285866	179.103901	47.371354
2372.820811	164.268553	47.376359
2369.509365	174.463110	47.381364
2365.889530	171.094871	47.386369
2362.370102	162.816593	47.391373
2358.921358	171.542763	47.396378
2355.447463	167.424332	47.401383
2351.775594	170.810685	47.406388
2348.405950	163.920213	47.411393
2345.244531	167.304176	47.416397
2341.459959	168.946677	47.421402
2338.094385	156.437213	47.426407
2334.457834	158.947379	47.431412
2331.065224	169.516225	47.436417
2328.000169	155.260768	47.441421
2324.233100	167.901149	47.446426
2320.730988	157.593391	47.451431
2316.771792	153.307189	47.456436
2313.384104	160.686867	47.461441
2310.131411	154.642370	47.466445
2306.480721	159.191790	47.471450
2302.869844	159.046280	47.476455
2299.651707	159.270395	47.481460
2296.136447	162.685995	47.486465
2292.813796	156.754070	47.491469
2288.938126	159.536824	47.496474
2285.532649	157.605957	47.501479
2282.529827	153.355614	47.506484
2278.752694	151.164419	47.511489
2275.446088	151.100154	47.516493
2271.276065	158.330854	47.521498
2267.830581	153.705218	47.526503
2264.185817	151.349638	47.531508
2261.149242	146.471583	47.536513
2258.349658	147.100543	47.541517
2254.791532	159.212400	47.546522
2251.065313	158.210539	47.551527
2247.405444	151.341551	47.556532
2243.692726	150.228549	47.561537
2240.280808	151.763168	47.566541
2236.526710	165.444756	47.571546
2233.096262	158.342689	47.576551
2230.182882	153.220076	47.581556
2226.436135	155.298779	47.586561
2223.175427	148.261564	47.591565
2219.505501	151.001735	47.596570
2215.639816	152.949999	47.601575
2212.372167	140.257936	47.606580
2208.350030	146.147571	47.611585
2204.874640	143.817264	47.616589
2201.896745	156.373395	47.621594
2198.385998	143.510994	47.626599
2194.908628	152.700795	47.631604
2191.515492	148.759742	47.636609
2188.145197	149.093255	47.641613
2184.098038	157.114606	47.646618
2180.687677	150.174709	47.651623
2177.245561	140.416446	47.656628
2173.581873	144.594247	47.661633
2170.293224	148.580061	47.666637
2166.937476	148.512111	47.671642
2163.669653	148.554463	47.676647
2159.816980	149.905697	47.681652
2156.144485	143.768526	47.686657
2153.026221	148.451286	47.691661
2148.851960	156.666960	47.696666
2145.766632	151.361815	47.701671
2142.433119	155.814692	47.706676
2139.045359	151.376228	47.711681
2135.375120	146.583215	47.716685
2131.638204	159.827608	47.721690
2128.492677	155.083309	47.726695
2125.369299	150.455229	47.731700
2121.855449	141.953703	47.736705
2117.968130	140.321517	47.741709
2114.528894	151.063565	47.746714
2110.933060	147.470313	47.751719
2107.368181	148.588526	47.756724
2104.013495	143.832866	47.761729
2100.227359	143.311272	47.766733
2096.662755	148.322510	47.771738
2093.272759	146.731627	47.776743
2089.868443	143.713447	47.781748
2086.219145	151.258202	47.786753
2082.815832	142.967450	47.791757
2079.131305	150.531929	47.796762
2075.622202	139.665986	47.801767
2072.158051	136.614080	47.806772
2069.187108	148.287186	47.811777
2065.784681	143.409684	47.816781
2062.113153	152.287046	47.821786
2058.764236	148.520593	47.826791
2055.166810	139.018189	47.831796
2051.611507	145.142455	47.836801
2048.258851	140.759320	47.841805
2044.209991	153.784872	47.846810
2041.201220	139.967822	47.851815
2037.033119	144.330903	47.856820
2033.586248	143.008606	47.861825
2030.228331	147.279482	47.866829
2026.574736	148.718801	47.871834
2023.293923	139.828751	47.876839
2020.017120	138.320455	47.881844
2016.464133	138.362458	47.886849
2013.187847	142.852215	47.891853
2009.773179	138.405336	47.896858
2006.462128	135.784896	47.901863
2002.728611	143.626626	47.906868
1998.389613	136.104524	47.911873
1995.549392	133.531125	47.916877
1991.821671	135.389358	47.921882
1988.140688	143.786260	47.926887
1984.958490	134.873257	47.931892
1981.536832	134.239606	47.936897
1978.180818	127.986502	47.941901
1973.928545	135.944993	47.946906
1970.783154	131.314113	47.951911
1967.601493	138.859904	47.956916
1963.901022	144.887891	47.961921
1960.750751	144.405119	47.966925
1956.825915	141.578833	47.971930
1953.526718	137.696596	47.976935
1949.888965	130.363306	47.981940
1946.303149	138.620707	47.986945
1942.852916	131.791016	47.991949
1939.343115	147.429633	47.996954
1935.958246	140.646380	48.001959
1932.590387	132.170705	48.006964
1927.951128	142.068753	48.011969
1924.925857	140.530647	48.016973
1921.717777	139.216860	48.021978
1918.261430	138.409305	48.026983
1915.193785	139.730011	48.031988
1911.597888	131.872177	48.036993
1908.225736	136.873448	48.041997
1904.529460	136.118900	48.047002
1901.176613	127.103475	48.052007
1897.637671	129.794559	48.057012
1894.093776	143.480346	48.062017
1890.573424	133.125352	48.067021
1886.588975	124.345451	48.072026
1883.082099	132.804630	48.077031
1880.109231	134.967251	48.082036
1876.076467	136.918880	48.087041
1872.962738	130.968499	48.092045
1869.591084	138.479569	48.097050
1865.908848	135.052539	48.102055
1862.459433	146.305133	48.107060
1859.090057	140.345431	48.112065
1855.368003	132.217697	48.117069
1851.861017	135.148499	48.122074
1848.601788	133.353150	48.127079
1844.859455	127.792699	48.132084
1841.052488	135.873131	48.137089
1837.737963	139.349634	48.142093
1833.995354	138.777094	48.147098
1830.637397	133.160239	48.152103
1827.849795	128.140387	48.157108
1824.026119	132.185702	48.162113
1820.811195	133.112434	48.167117
1816.747293	134.814004	48.172122
1813.260383	137.544195	48.177127
1809.893790	135.242406	48.182132
1806.162145	139.517023	48.187137
1802.868028	130.080064	48.192141
1799.338156	139.057673	48.197146
1795.921422	129.217311	48.202151
1792.778581	128.102568	48.207156
1788.942758	133.954460	48.212161
1785.238868	138.435832	48.217165
1781.747413	138.985555	48.222170
1778.022082	144.722836	48.227175
1775.079022	136.034794	48.232180
1771.559083	136.140721	48.237185
1767.746935	125.047152	48.242189
1764.385678	131.735314	48.247194
1760.774953	137.619930	48.252199
1757.215700	128.691029	48.257204
1753.750042	133.259291	48.262209
1750.467075	128.837780	48.267213
1746.796275	132.420755	48.272218
1743.304827	127.242902	48.277223
1740.167156	130.394783	48.282228
1736.490185	127.054960	48.287233
1732.853084	129.457955	48.292237
1729.058698	134.247891	48.297242
1725.424515	133.986148	48.302247
1722.764330	121.413176	48.307252
1718.882558	122.600238	48.312257
1715.620744	132.024076	48.317261
1711.644172	124.249103	48.322266
1707.971270	132.136398	48.327271
1704.830885	122.296568	48.332276
1700.970456	119.669948	48.337281
1697.633998	124.083232	48.342285
1694.421862	134.181496	48.347290
1691.001152	140.189783	48.352295
1687.456075	127.413881	48.357300
1683.991154	118.890832	48.362305
1680.632884	121.968243	48.367309
1676.560118	119.907650	48.372314
1673.132899	131.864016	48.377319
1669.827945	127.645365	48.382324
1666.256370	125.867901	48.387329
1662.714421	119.720629	48.392333
1658.831506	120.899327	48.397338
1655.400090	122.822486	48.402343
1652.434104	127.362208	48.407348
1648.928721	128.286529	48.412353
1645.883420	117.051117	48.417357
1642.625151	117.151519	48.422362
1638.523840	120.771939	48.427367
1634.890209	122.367782	48.432372
1630.968757	132.947061	48.437377
1627.346836	127.977856	48.442381
1624.140945	126.732906	48.447386
1620.313368	134.504978	48.452391
1617.728809	119.245459	48.457396
1613.822116	127.265391	48.462401
1610.349873	116.865542	48.467405
1606.651972	130.595576	48.472410
1602.978892	132.022925	48.477415
1599.848263	130.790824	48.482420
1595.859083	120.902782	48.487425
1592.839880	118.406940	48.492429
1589.298967	129.949482	48.497434
1585.846038	128.182177	48.502439
1582.621593	123.828640	48.507444
1578.890168	131.607751	48.512449
1575.551478	118.299647	48.517453
1571.728120	119.641709	48.522458
1567.407757	117.362865	48.527463
1564.586312	115.660168	48.532468
1560.918113	125.964751	48.537473
1557.873431	118.235485	48.542477
1554.353908	110.403252	48.547482
1550.631820	124.397156	48.552487
1546.928600	114.104722	48.557492
1543.321653	115.493464	48.562497
1540.313138	134.349178	48.567501
1536.710851	132.257789	48.572506
1533.292298	118.315498	48.577511
1529.800247	112.468277	48.582516
1525.867140	118.289578	48.587521
1522.507554	118.279683	48.592525
1519.125731	116.907445	48.597530
1514.996564	121.574355	48.602535
1512.014104	113.094618	48.607540
1508.659982	120.000128	48.612545
1505.295015	120.268654	48.617549
1501.627536	122.799011	48.622554
1498.183320	125.117111	48.627559
1494.777034	117.195188	48.632564
1490.956933	123.058139	48.637569
1488.024086	123.977238	48.642573
1484.420216	116.236605	48.647578
1480.730664	116.432033	48.652583
1477.219297	112.461735	48.657588
1473.491605	124.996363	48.662593
1470.001744	123.155102	48.667597
1466.793064	125.992157	48.672602
1463.194568	128.691199	48.677607
1459.736034	115.232073	48.682612
1455.814709	115.111880	48.687617
1452.677490	112.659356	48.692621
1448.990435	119.556794	48.697626
1445.608860	116.706166	48.702631
1442.264699	111.858850	48.707636
1438.431180	115.156671	48.712641
1435.303941	109.062043	48.717645
1431.846166	120.522349	48.722650
1427.706658	118.356603	48.727655
1424.357763	110.178903	48.732660
1420.914921	117.423970	48.737665
1417.611878	107.011710	48.742669
1414.237162	112.522183	48.747674
1410.521753	119.855255	48.752679
1406.888057	111.215397	48.757684
1403.830580	116.097259	48.762689
1400.398022	111.093877	48.767693
1396.785059	115.402962	48.772698
1393.039238	121.543063	48.777703
1389.449145	117.389377	48.782708
1385.933556	120.943255	48.787713
1382.410892	109.442171	48.792717
1379.250035	119.695645	48.797722
1375.481678	120.356282	48.802727
1372.025245	116.435083	48.807732
1368.331958	121.725765	48.812737
1365.095729	106.880577	48.817741
1361.749333	112.141235	48.822746
1358.126385	114.207725	48.827751
1354.767605	109.579915	48.832756
1350.958269	115.661950	48.837761
1347.645923	107.341425	48.842765
1344.039081	108.906846	48.847770
1340.362340	114.037153	48.852775
1337.097629	111.464943	48.857780
1333.629473	128.370037	48.862785
1330.153487	115.699879	48.867789
1326.230719	115.837197	48.872794
1322.607644	121.445630	48.877799
1319.828351	108.603863	48.882804
1315.974096	109.403807	48.887809
1312.794301	110.133373	48.892813
1308.880760	112.861304	48.897818
1305.270017	114.382795	48.902823
1302.124713	106.527026	48.907828
1298.026868	117.164957	48.912833
1294.736570	111.326299	48.917837
1291.746376	104.113930	48.922842
1287.846411	97.421008	48.927847
1284.797255	105.176217	48.932852
1281.140201	116.563413	48.937857
1277.748841	117.489220	48.942861
1274.160713	117.037792	48.947866
1270.568826	110.182737	48.952871
1267.061058	97.751698	48.957876
1263.317954	113.489191	48.962881
1259.619601	116.318961	48.967885
1256.523167	118.859658	48.972890
1252.808745	115.411255	48.977895
1249.633289	109.201557	48.982900
1245.689825	111.360374	48.987905
1242.480455	107.178164	48.992909
1238.764919	114.700853	48.997914
1234.958882	118.926851	49.002919
1232.442521	117.912385	49.007924
1228.850140	114.218123	49.012929
1225.130253	108.211368	49.017933
1221.361265	100.593560	49.022938
1217.551502	113.444410	49.027943
1214.503087	109.388958	49.032948
1210.794029	108.309544	49.037953
1207.361568	102.741935	49.042957
1204.028696	97.814355	49.047962
1200.367583	119.170589	49.052967
1196.625430	103.009668	49.057972
1193.503090	105.532962	49.062977
1189.779349	104.088387	49.067981
1186.496368	115.599247	49.072986
1182.795988	114.149141	49.077991
1179.990966	108.796041	49.082996
1176.249386	104.790216	49.088001
1172.232786	106.898794	49.093005
1168.430015	104.983855	49.098010
1165.085815	109.189192	49.103015
1162.064359	110.779617	49.108020
1158.343953	112.998541	49.113025
1154.941961	107.930660	49.118029
1151.534079	101.932825	49.123034
1148.031813	110.454769	49.128039
1144.371125	89.744980	49.133044
1140.645322	107.129993	49.138049
1137.246377	113.375833	49.143053
1133.945027	107.489759	49.148058
1130.362317	107.123443	49.153063
1126.910520	103.540502	49.158068
1123.418262	101.654933	49.163073
1119.740459	103.644864	49.168077
1116.502162	106.572689	49.173082
1112.573045	111.096885	49.178087
1109.167008	111.739288	49.183092
1105.402281	116.044759	49.188097
1102.133128	106.902828	49.193101
1098.800357	110.467699	49.198106
1095.301859	110.380116	49.203111
1091.682381	95.023803	49.208116
1088.558879	100.529936	49.213121
1084.719230	110.381465	49.218125
1081.696051	103.842559	49.223130
1077.852554	108.038908	49.228135
1074.248580	111.462102	49.233140
1070.393638	110.459926	49.238145
1067.187906	104.740324	49.243149
1063.827851	117.278939	49.248154
1060.048943	112.938087	49.253159
1056.766044	108.258447	49.258164
1053.581340	112.292674	49.263169
1049.723542	107.484986	49.268173
1046.479223	107.539263	49.273178
1042.858634	107.274352	49.278183
1039.231536	104.630217	49.283188
1035.600662	113.278117	49.288193
1032.098618	103.472929	49.293197
1028.954762	101.963290	49.298202
1025.084842	104.957353	49.303207
1021.875475	93.013709	49.308212
1018.400630	104.657520	49.313217
1014.814766	108.803573	49.318221
1011.294077	94.516728	49.323226
1007.430847	103.688489	49.328231
1003.866557	105.804962	49.333236
1000.644976	103.816364	49.338241
997.101901	106.078113	49.343245
993.857994	95.762208	49.348250
990.083115	97.237656	49.353255
986.788251	101.937188	49.358260
983.207944	94.959940	49.363265
979.933602	105.169240	49.368269
976.458955	97.248654	49.373274
972.562911	110.957269	49.378279
969.415275	101.086899	49.383284
965.853233	114.124753	49.388289
961.872513	109.275951	49.393293
958.480847	107.347913	49.398298
955.176620	105.972225	49.403303
951.641234	114.019953	49.408308
948.006267	112.224927	49.413313
944.467032	102.113094	49.418317
941.530027	95.204871	49.423322
937.455559	104.810610	49.428327
934.609279	104.442674	49.433332
930.759038	109.012249	49.438337
927.056143	116.526287	49.443341
923.588542	95.683752	49.448346
920.080329	109.384883	49.453351
916.802088	102.769394	49.458356
912.982035	108.528434	49.463361
909.643760	106.185139	49.468365
906.405945	109.153231	49.473370
902.520113	107.678063	49.478375
898.983262	106.581043	49.483380
895.340607	96.463334	49.488385
891.934000	104.071909	49.493389
888.617725	97.381424	49.498394
885.182778	109.018505	49.503399
881.973202	103.231761	49.508404
878.291948	104.215200	49.513409
875.023278	101.284373	49.518413
870.979706	90.157721	49.523418
867.433707	108.064834	49.528423
863.898393	97.388879	49.533428
860.917984	106.706173	49.538433
856.962513	118.852263	49.543437
853.560665	96.833486	49.548442
849.775151	104.934098	49.553447
846.826873	106.478932	49.558452
843.108305	108.078941	49.563457
839.141527	105.441877	49.568461
836.199985	103.786357	49.573466
832.385755	109.660497	49.578471
829.426411	102.461821	49.583476
825.717554	98.246781	49.588481
821.842074	107.541805	49.593485
818.464854	103.094916	49.598490
814.485254	100.712744	49.603495
811.804198	86.992692	49.608500
808.337581	102.773680	49.613505
804.296680	100.698298	49.618509
800.944551	93.521193	49.623514
797.418734	109.929657	49.628519
793.502475	103.628746	49.633524
790.884754	96.811619	49.638529
787.231028	96.666662	49.643533
783.798313	97.709344	49.648538
780.001801	96.589070	49.653543
776.523253	104.018080	49.658548
773.168104	93.263995	49.663553
769.625014	98.255595	49.668557
766.069781	89.239447	49.673562
762.444641	103.441681	49.678567
758.954723	104.286841	49.683572
755.279492	99.627562	49.688577
751.763886	90.921961	49.693581
748.346909	95.295476	49.698586
744.878676	83.256046	49.703591
741.565876	97.197551	49.708596
737.882694	100.184017	49.713601
734.363562	100.721469	49.718605
731.534858	94.476596	49.723610
727.489676	97.610061	49.728615
724.428240	91.526256	49.733620
720.642604	91.920278	49.738625
716.774736	99.815732	49.743629
713.289813	94.333825	49.748634
709.823060	98.416946	49.753639
706.172964	91.531306	49.758644
702.636770	83.676304	49.763649
699.438269	93.950920	49.768653
696.018485	93.741827	49.773658
692.041401	99.193351	49.778663
689.010424	81.378402	49.783668
685.700910	95.487987	49.788673
682.144468	97.494707	49.793677
678.751890	91.647241	49.798682
675.021913	108.973330	49.803687
671.193043	93.753117	49.808692
667.718767	97.871536	49.813697
664.206762	96.508805	49.818701
661.372604	85.550168	49.823706
657.417119	101.431972	49.828711
653.606530	104.569456	49.833716
650.313544	94.026270	49.838721
646.629771	93.342459	49.843725
643.472389	94.913724	49.848730
639.932202	95.225524	49.853735
636.522481	99.970718	49.858740
633.064086	94.534891	49.863745
629.372336	97.533681	49.868749
625.897411	87.754174	49.873754
622.472476	91.963713	49.878759
618.637494	84.263278	49.883764
615.214458	84.856843	49.888769
611.842611	97.135128	49.893773
608.431022	93.872686	49.898778
604.754027	95.643441	49.903783
601.341752	80.992204	49.908788
597.969865	93.584226	49.913793
594.083646	92.176495	49.918797
590.612064	91.057519	49.923802
587.061332	100.839655	49.928807
584.279245	92.288457	49.933812
580.520218	93.047534	49.938817
576.898992	89.630512	49.943821
573.149347	91.781271	49.948826
569.576173	99.314693	49.953831
566.367873	94.107325	49.958836
562.991732	97.866065	49.963841
559.214225	91.176973	49.968845
555.971032	95.456269	49.973850
552.625125	95.952183	49.978855
548.595314	91.296843	49.983860
545.332646	89.874942	49.988865
541.516589	102.193874	49.993869
538.331061	91.116346	49.998874
535.080246	94.746171	50.003879
531.372938	92.045334	50.008884
528.253935	90.991280	50.013889
524.227471	93.015042	50.018893
520.842750	89.920663	50.023898
517.004971	92.312822	50.028903
513.545162	86.923670	50.033908
509.958171	88.326715	50.038913
506.706937	89.571898	50.043917
503.211942	90.309606	50.048922
499.681024	91.529069	50.053927
496.093941	87.116339	50.058932
492.576951	93.203286	50.063937
489.338600	94.139825	50.068941
485.969445	90.579702	50.073946
482.317841	98.168146	50.078951
478.711959	101.523189	50.083956
475.400111	103.241396	50.088961
471.841394	103.317795	50.093965
468.200523	95.900105	50.098970
464.309652	99.938762	50.103975
461.121716	102.853929	50.108980
457.821775	97.440864	50.113985
453.916706	88.974110	50.118989
450.701976	80.338674	50.123994
447.126504	103.065324	50.128999
443.698118	76.998559	50.134004
440.110862	85.827351	50.139009
436.892558	87.638250	50.144013
433.410997	88.897739	50.149018
429.403309	88.727002	50.154023
426.084911	88.872448	50.159028
422.642294	102.438620	50.164033
418.965750	100.953049	50.169037
415.731962	90.224229	50.174042
412.426883	84.661395	50.179047
408.914785	86.590885	50.184052
405.369591	81.872363	50.189057
401.502491	93.149094	50.194061
398.483597	82.758994	50.199066
394.374815	89.002151	50.204071
390.679518	79.456713	50.209076
387.869095	86.896671	50.214081
384.450605	89.369697	50.219085
380.887148	87.524512	50.224090
377.022309	100.375342	50.229095
373.457556	87.625197	50.234100
369.986744	89.269677	50.239105
366.354012	89.291176	50.244109
363.372867	80.824777	50.249114
359.533944	88.889457	50.254119
355.675459	82.300204	50.259124
353.051985	90.199318	50.264129
349.119791	96.443717	50.269133
346.056508	82.819627	50.274138
342.303340	83.303509	50.279143
338.464274	75.369042	50.284148
335.235611	79.337634	50.289153
331.032733	80.600418	50.294157
327.853570	80.402280	50.299162
324.190652	94.616547	50.304167
321.309957	85.258690	50.309172
317.821640	78.937527	50.314177
314.429614	93.938519	50.319181
310.760438	75.898366	50.324186
306.838220	98.229405	50.329191
303.423646	73.921789	50.334196
299.591311	78.533427	50.339201
296.192873	92.940094	50.344205
293.124939	93.888234	50.349210
289.746823	93.034560	50.354215
286.501813	87.077904	50.359220
283.112738	83.541411	50.364225
279.210273	89.689973	50.369229
275.519398	89.396550	50.374234
271.389202	94.586314	50.379239
268.214406	89.470358	50.384244
265.223723	85.940964	50.389249
261.444293	87.407013	50.394253
258.174522	90.406429	50.399258
254.664088	96.895321	50.404263
250.980857	92.541241	50.409268
247.281034	87.895812	50.414273
243.501977	85.254063	50.419277
240.736822	93.274391	50.424282
236.912360	92.582391	50.429287
233.437561	92.375232	50.434292
230.362745	84.080949	50.439297
226.439901	88.143763	50.444301
223.011960	91.993602	50.449306
219.096622	92.925216	50.454311
215.512685	96.413409	50.459316
212.040025	87.247336	50.464321
208.531838	90.507749	50.469325
205.599030	84.872281	50.474330
202.209640	86.833104	50.479335
198.806013	87.476953	50.484340
195.600084	87.223024	50.489345
191.673090	92.732548	50.494349
187.985178	86.064415	50.499354
184.287652	97.277324	50.504359
180.963832	89.614961	50.509364
177.701043	89.506680	50.514369
173.701709	95.432855	50.519373
170.643475	81.547787	50.524378
166.596390	94.313196	50.529383
163.309636	92.313007	50.534388
159.904380	80.018697	50.539393
156.168270	84.228673	50.544397
152.657323	80.028607	50.549402
149.578696	90.920942	50.554407
146.164927	92.586204	50.559412
142.611102	96.533736	50.564417
138.715701	98.499572	50.569421
135.698589	85.196903	50.574426
131.942097	85.995972	50.579431
128.385628	87.064768	50.584436
125.020152	81.957710	50.589441
120.845318	86.327015	50.594445
117.936039	84.383854	50.599450
114.341874	83.657329	50.604455
110.633351	76.645782	50.609460
107.463128	78.772486	50.614465
104.009242	83.482115	50.619469
100.130690	84.890742	50.624474
96.958187	89.178001	50.629479
93.376184	78.682634	50.634484
89.780891	77.592171	50.639489
85.999954	88.588442	50.644493
82.859334	85.175666	50.649498
79.146064	76.842539	50.654503
76.053008	82.920800	50.659508
72.777284	83.167307	50.664513
69.189139	91.378242	50.669517
65.757203	80.934356	50.674522
61.435166	88.521515	50.679527
58.162833	80.873808	50.684532
54.524933	78.489233	50.689537
50.996498	85.509101	50.694541
47.785304	75.498554	50.699546
44.220225	82.748724	50.704551
41.137967	76.314165	50.709556
37.634880	76.618387	50.714561
33.734676	90.195105	50.719565
30.225740	89.707696	50.724570
27.061371	89.098433	50.729575
23.346398	79.481321	50.734580
19.771841	78.596524	50.739585
16.246143	91.191694	50.744589
12.711659	82.446674	50.749594
9.075990	74.672977	50.754599
5.228496	79.240521	50.759604
2.324336	81.198706	50.764609