Fri Jun 17 17:29:47 2022

Number of Points = 9926

Depth (nm)	Load (N)	Time (s)
1.423306	96.433345	0.000000
1.171921	94.225870	0.005005
1.506431	106.606241	0.010010
1.411841	106.379568	0.015014
1.501344	95.523609	0.020019
1.186568	93.541171	0.025024
0.946175	79.151187	0.030029
0.909907	74.881958	0.035034
0.439297	78.726376	0.040038
0.408507	47.950707	0.045043
0.341828	46.639797	0.050048
0.076725	39.028136	0.055053
0.020905	28.290901	0.060058
-0.469574	34.138953	0.065062
-0.895628	19.667406	0.070067
-1.493824	14.655702	0.075072
-1.238172	6.933623	0.080077
-1.449348	-2.213135	0.085082
-2.291975	-2.579499	0.090086
-2.532065	-11.990999	0.095091
-2.398348	-4.563879	0.100096
-2.738806	-27.347349	0.105101
-2.981657	-26.507079	0.110106
-3.464100	-23.240869	0.115110
-3.022707	-29.411610	0.120115
-3.935035	-31.152236	0.125120
-4.328327	-31.371487	0.130125
-4.387869	-34.549725	0.135130
-5.013032	-25.512161	0.140134
-5.390315	-45.512259	0.145139
-5.885695	-30.937093	0.150144
-5.955370	-33.135285	0.155149
-5.847288	-27.752398	0.160154
-6.273745	-29.775060	0.165158
-6.422006	-32.033795	0.170163
-6.396661	-33.198379	0.175168
-6.510908	-38.446988	0.180173
-7.013134	-32.338900	0.185178
-7.381822	-34.692614	0.190182
-7.410645	-44.810328	0.195187
-7.910359	-37.714234	0.200192
-8.023769	-28.578611	0.205197
-8.013393	-33.893321	0.210202
-8.950840	-28.194573	0.215206
-9.151940	-21.932099	0.220211
-9.246664	-32.165947	0.225216
-9.564967	-25.898794	0.230221
-9.456065	-26.552370	0.235226
-9.718432	-29.023803	0.240230
-9.631959	-20.606135	0.245235
-10.381156	-32.482898	0.250240
-11.027798	-19.293291	0.255245
-10.833681	-31.850367	0.260250
-11.166164	-20.062519	0.265254
-10.764331	-25.089670	0.270259
-11.593303	-25.313855	0.275264
-12.380605	-22.558178	0.280269
-12.393317	-32.811972	0.285274
-13.020641	-18.858751	0.290278
-12.945396	-33.034894	0.295283
-12.748870	-21.779365	0.300288
-12.674154	-26.531331	0.305293
-12.618211	-27.749151	0.310298
-13.456575	-18.520451	0.315302
-13.624392	-27.547516	0.320307
-13.862584	-26.715123	0.325312
-14.107393	-23.841238	0.330317
-15.354522	-28.570028	0.335322
-15.723283	-18.968288	0.340326
-14.650275	-29.179963	0.345331
-15.219550	-27.476381	0.350336
-15.527445	-30.254593	0.355341
-15.467436	-30.610165	0.360346
-15.789816	-29.005242	0.365350
-16.538448	-31.795244	0.370355
-17.097003	-21.733555	0.375360
-17.589196	-26.308411	0.380365
-17.335499	-27.272775	0.385370
-17.377076	-25.088596	0.390374
-17.192480	-32.493772	0.395379
-17.632271	-28.638715	0.400384
-18.066392	-20.600411	0.405389
-18.726035	-29.823169	0.410394
-18.946202	-20.521010	0.415398
-18.749364	-30.189033	0.420403
-18.639497	-21.138077	0.425408
-19.014926	-38.148344	0.430413
-19.596680	-31.886537	0.435418
-20.307526	-24.517757	0.440422
-20.165090	-23.616815	0.445427
-20.956551	-23.760803	0.450432
-20.747399	-19.833448	0.455437
-20.373466	-24.778609	0.460442
-21.062024	-25.944506	0.465446
-20.852913	-34.091573	0.470451
-21.529958	-33.857945	0.475456
-21.912309	-31.429265	0.480461
-21.963047	-28.457598	0.485466
-22.461544	-22.180618	0.490470
-22.443341	-30.412774	0.495475
-23.062689	-36.472512	0.500480
-23.490708	-19.454735	0.505485
-23.650947	-26.535409	0.510490
-24.017467	-25.411343	0.515494
-23.884665	-27.801845	0.520499
-24.159418	-28.717047	0.525504
-24.052063	-26.402917	0.530509
-24.481529	-34.333531	0.535514
-25.260549	-28.704920	0.540518
-25.294251	-27.593158	0.545523
-25.606703	-23.437223	0.550528
-25.779015	-31.064861	0.555533
-25.593605	-29.497181	0.560538
-25.855456	-23.768846	0.565542
-26.588503	-29.666623	0.570547
-26.766308	-26.413951	0.575552
-27.104761	-26.610346	0.580557
-27.033078	-33.480537	0.585562
-27.405317	-23.681880	0.590566
-27.443694	-35.603184	0.595571
-27.851955	-30.301809	0.600576
-28.425618	-27.630776	0.605581
-28.847008	-27.023868	0.610586
-29.115504	-28.783104	0.615590
-28.771804	-34.253265	0.620595
-28.844314	-35.972459	0.625600
-29.054113	-25.435558	0.630605
-29.024941	-33.682164	0.635610
-30.124017	-21.781692	0.640614
-30.322021	-30.072627	0.645619
-30.093295	-28.996593	0.650624
-30.611189	-21.716123	0.655629
-30.907209	-35.737211	0.660634
-31.647844	-21.482975	0.665638
-31.868139	-38.467916	0.670643
-31.774005	-35.928213	0.675648
-31.723027	-23.247453	0.680653
-31.440886	-29.018770	0.685658
-31.928572	-21.198887	0.690662
-32.457935	-32.298001	0.695667
-32.904529	-28.614080	0.700672
-33.003183	-18.819654	0.705677
-33.018645	-35.442013	0.710682
-33.855273	-28.051141	0.715686
-34.294914	-32.342086	0.720691
-34.648462	-30.720734	0.725696
-34.747260	-29.328598	0.730701
-34.537543	-32.671175	0.735706
-35.003934	-16.865726	0.740710
-34.788878	-21.593464	0.745715
-34.768597	-23.393992	0.750720
-36.354921	-24.246871	0.755725
-36.107777	-23.308873	0.760730
-36.605219	-25.911722	0.765734
-36.344861	-29.987313	0.770739
-36.683654	-15.588330	0.775744
-36.680550	-22.020498	0.780749
-36.727251	-25.796019	0.785754
-37.778718	-26.561785	0.790758
-37.735483	-37.276562	0.795763
-37.954214	-30.434168	0.800768
-38.280973	-23.406676	0.805773
-37.879113	-34.319988	0.810778
-38.625092	-19.905616	0.815782
-38.847701	-22.831596	0.820787
-39.328785	-27.856036	0.825792
-39.709013	-18.682964	0.830797
-39.476265	-26.275125	0.835802
-39.615029	-20.526204	0.840806
-40.076573	-25.774507	0.845811
-40.614938	-32.136990	0.850816
-41.074933	-19.611442	0.855821
-41.115028	-23.495211	0.860826
-41.382724	-19.731902	0.865830
-40.853866	-20.629332	0.870835
-41.299243	-17.797090	0.875840
-42.328005	-22.264991	0.880845
-42.441697	-26.081668	0.885850
-42.843285	-28.280531	0.890854
-42.759099	-17.383625	0.895859
-42.831111	-23.361682	0.900864
-43.089521	-15.781775	0.905869
-42.944852	-23.083232	0.910874
-43.765544	-24.755215	0.915878
-44.364201	-25.005048	0.920883
-44.530423	-24.905069	0.925888
-44.565888	-31.013713	0.930893
-44.727710	-23.211294	0.935898
-44.759856	-23.173068	0.940902
-44.906735	-20.129377	0.945907
-45.720014	-25.035846	0.950912
-46.160392	-17.944078	0.955917
-45.699021	-23.898714	0.960922
-46.688694	-27.521827	0.965926
-46.358166	-27.775750	0.970931
-46.130390	-25.932735	0.975936
-46.788057	-20.418811	0.980941
-47.090989	-27.754393	0.985946
-47.438888	-28.264353	0.990950
-47.924328	-22.180755	0.995955
-47.914192	-26.812860	1.000960
-48.057374	-25.535099	1.005965
-47.942562	-22.089535	1.010970
-48.718414	-30.357425	1.015974
-48.910379	-17.749349	1.020979
-49.227017	-18.681661	1.025984
-49.330118	-25.763740	1.030989
-49.413797	-27.789505	1.035994
-50.659321	-23.056574	1.040998
-50.647178	-31.050134	1.046003
-50.943966	-28.525959	1.051008
-51.098009	-21.964065	1.056013
-50.547040	-31.821190	1.061018
-51.248241	-15.240471	1.066022
-50.761003	-24.327483	1.071027
-51.115919	-26.965861	1.076032
-51.942551	-22.770628	1.081037
-52.130448	-29.730868	1.086042
-52.460884	-21.242917	1.091046
-52.658580	-17.824928	1.096051
-53.181554	-31.798421	1.101056
-53.780511	-30.585199	1.106061
-53.831191	-30.239806	1.111066
-53.920356	-26.186107	1.116070
-53.901883	-23.016577	1.121075
-53.688603	-30.515714	1.126080
-53.973514	-34.483892	1.131085
-54.383139	-27.018762	1.136090
-55.000610	-31.272250	1.141094
-54.962631	-34.668763	1.146099
-55.049554	-20.917851	1.151104
-55.900643	-22.104083	1.156109
-56.119373	-32.788141	1.161114
-57.007397	-22.065880	1.166118
-57.205224	-23.231255	1.171123
-56.845760	-23.296803	1.176128
-57.269572	-14.759385	1.181133
-57.064147	-27.606837	1.186138
-57.036498	-23.333588	1.191142
-57.005701	-33.090431	1.196147
-57.826710	-26.514558	1.201152
-58.678531	-16.353203	1.206157
-58.397343	-26.815294	1.211162
-58.513103	-21.733424	1.216166
-58.635450	-21.677244	1.221171
-59.134052	-24.338307	1.226176
-59.761943	-22.354632	1.231181
-59.975778	-23.206946	1.236186
-60.386391	-14.223585	1.241190
-60.677649	-23.244926	1.246195
-60.592154	-29.672039	1.251200
-60.695482	-23.308802	1.256205
-60.329550	-23.927555	1.261210
-61.030243	-26.253700	1.266214
-61.469868	-12.580902	1.271219
-61.470179	-22.777362	1.276224
-61.814243	-11.492552	1.281229
-61.532684	-29.229080	1.286234
-62.851075	-27.301116	1.291238
-62.910711	-28.708301	1.296243
-63.684676	-29.192621	1.301248
-63.992727	-27.767871	1.306253
-63.857474	-31.683746	1.311258
-64.148993	-20.824832	1.316262
-63.691793	-25.003791	1.321267
-63.876469	-25.648427	1.326272
-64.088302	-26.652622	1.331277
-64.485855	-32.972204	1.336282
-65.007265	-36.168972	1.341286
-65.367047	-18.618304	1.346291
-65.522281	-27.791701	1.351296
-65.456201	-15.660646	1.356301
-65.779857	-36.560596	1.361306
-66.324553	-30.330991	1.366310
-66.739623	-27.661454	1.371315
-66.937940	-25.511997	1.376320
-67.245362	-19.603026	1.381325
-66.851251	-32.606946	1.386330
-67.090535	-23.939582	1.391334
-67.797002	-37.270248	1.396339
-67.630764	-30.670236	1.401344
-68.102855	-19.819784	1.406349
-68.337689	-23.639805	1.411354
-69.218174	-17.855989	1.416358
-69.571211	-28.391232	1.421363
-69.612032	-19.352132	1.426368
-69.882462	-25.425664	1.431373
-69.743519	-25.680300	1.436378
-69.516374	-34.742620	1.441382
-70.008226	-20.762587	1.446387
-69.875780	-24.264196	1.451392
-70.947427	-22.871360	1.456397
-71.190553	-32.319034	1.461402
-71.519484	-29.566334	1.466406
-71.284434	-25.068272	1.471411
-71.122918	-34.305764	1.476416
-72.301063	-29.254488	1.481421
-72.581008	-31.440022	1.486426
-72.853200	-31.005317	1.491430
-73.200901	-33.012054	1.496435
-72.879871	-32.681882	1.501440
-73.163718	-34.061661	1.506445
-73.014205	-31.501369	1.511450
-73.573414	-23.997952	1.516454
-74.457384	-25.024006	1.521459
-74.641485	-25.246056	1.526464
-74.900947	-31.322986	1.531469
-74.716219	-35.828615	1.536474
-75.025825	-29.462664	1.541478
-74.870107	-26.407512	1.546483
-75.055647	-30.513762	1.551488
-76.109120	-31.385939	1.556493
-76.346936	-37.375101	1.561498
-76.586136	-32.645077	1.566502
-76.665238	-34.561095	1.571507
-76.432845	-45.522791	1.576512
-76.602104	-32.790832	1.581517
-76.973588	-38.018576	1.586522
-77.625831	-35.113071	1.591526
-78.003018	-37.760963	1.596531
-78.046913	-34.916530	1.601536
-78.230125	-41.267001	1.606541
-78.300110	-38.798091	1.611546
-78.699964	-42.857266	1.616550
-79.387482	-25.762223	1.621555
-79.604403	-36.265031	1.626560
-79.759978	-32.132215	1.631565
-79.452664	-35.620464	1.636570
-79.826712	-30.569265	1.641574
-79.871912	-27.341793	1.646579
-80.583302	-27.384627	1.651584
-80.897955	-16.547124	1.656589
-80.772635	-28.738355	1.661594
-81.126619	-20.242147	1.666598
-81.536714	-28.885177	1.671603
-81.875640	-33.625009	1.676608
-82.508397	-25.416935	1.681613
-82.496625	-32.212638	1.686618
-82.663738	-23.681391	1.691622
-82.809353	-29.206963	1.696627
-82.588558	-29.631887	1.701632
-83.015673	-31.316798	1.706637
-83.628549	-32.155658	1.711642
-83.900474	-31.459731	1.716646
-84.382579	-24.843698	1.721651
-84.067373	-35.833769	1.726656
-84.176674	-22.314754	1.731661
-84.298686	-27.526549	1.736666
-85.135857	-28.186637	1.741670
-85.945967	-27.701975	1.746675
-85.822847	-31.138097	1.751680
-86.091918	-45.614541	1.756685
-86.272100	-41.218938	1.761690
-86.321337	-36.023814	1.766694
-86.151452	-22.207265	1.771699
-86.235960	-37.632575	1.776704
-87.022197	-14.252729	1.781709
-87.329631	-31.255936	1.786714
-87.226192	-20.515762	1.791718
-87.467470	-21.554527	1.796723
-88.281441	-25.736075	1.801728
-88.682981	-25.288746	1.806733
-88.835187	-25.289365	1.811738
-88.860171	-25.235359	1.816742
-89.126225	-25.441614	1.821747
-88.890267	-26.186760	1.826752
-89.415755	-25.642459	1.831757
-90.186332	-31.075779	1.836762
-90.621401	-21.319362	1.841766
-90.871790	-22.590843	1.846771
-90.659597	-30.427233	1.851776
-90.934394	-23.766927	1.856781
-90.739208	-30.097230	1.861786
-90.861212	-15.202090	1.866790
-91.289945	-29.408501	1.871795
-91.859745	-25.238593	1.876800
-92.415375	-16.678670	1.881805
-92.187837	-26.062707	1.886810
-92.574773	-25.701867	1.891814
-92.556137	-28.531591	1.896819
-92.668710	-26.328111	1.901824
-93.391037	-30.466482	1.906829
-93.829352	-33.974238	1.911834
-94.129162	-35.054774	1.916838
-94.266305	-31.695003	1.921843
-93.851062	-31.801400	1.926848
-94.216653	-27.064372	1.931853
-94.882095	-32.789259	1.936858
-95.334886	-28.402007	1.941862
-95.530830	-27.244922	1.946867
-95.662134	-34.644543	1.951872
-95.705976	-27.084724	1.956877
-95.972400	-29.586653	1.961882
-96.509993	-21.201407	1.966886
-97.128159	-18.100285	1.971891
-96.895099	-32.029943	1.976896
-97.172756	-21.339093	1.981901
-97.136793	-32.547758	1.986906
-97.418085	-16.029544	1.991910
-97.377453	-31.438958	1.996915
-98.305378	-21.017740	2.006912
-98.061850	-24.942842	2.016909
-97.162731	-23.370130	2.026906
-96.446977	-20.758077	2.036902
-96.061144	-22.309370	2.046899
-96.024492	-24.095431	2.056896
-95.711859	-26.603894	2.066893
-94.654748	-25.632609	2.076890
-94.362475	-25.098077	2.086886
-93.993282	-24.122880	2.096883
-93.280696	-22.444076	2.106880
-92.996323	-24.638822	2.116877
-92.125442	-25.308126	2.126874
-91.678020	-19.796594	2.136870
-91.520014	-20.704026	2.146867
-90.684748	-23.335134	2.156864
-90.256499	-20.730806	2.166861
-89.888834	-24.780078	2.176858
-88.783152	-24.147421	2.186854
-88.632518	-27.624770	2.196851
-88.341938	-19.395101	2.206848
-88.274495	-19.886978	2.216845
-87.658902	-19.524940	2.226842
-86.756092	-21.542323	2.236838
-85.867844	-19.708769	2.246835
-85.495196	-23.300675	2.256832
-85.402011	-22.518669	2.266829
-85.154480	-22.572015	2.276826
-84.103718	-22.429123	2.286822
-84.038407	-26.079991	2.296819
-82.841493	-19.779034	2.306816
-82.274518	-20.202011	2.316813
-82.817344	-21.746518	2.326810
-81.888706	-22.261427	2.336806
-81.324365	-23.804457	2.346803
-81.001673	-23.293949	2.356800
-79.969210	-25.432068	2.366797
-79.805817	-23.616719	2.376794
-79.568378	-24.030951	2.386790
-78.640213	-20.286294	2.396787
-78.122764	-25.244845	2.406784
-77.657024	-26.652933	2.416781
-77.410709	-17.494378	2.426778
-76.404515	-20.076445	2.436774
-76.407713	-22.213310	2.446771
-75.917938	-20.393336	2.456768
-74.999124	-21.631147	2.466765
-74.731499	-31.329271	2.476762
-74.464507	-25.042462	2.486758
-73.499220	-15.486942	2.496755
-73.198703	-20.034223	2.506752
-72.948102	-28.867860	2.516749
-72.258109	-22.551588	2.526746
-71.594622	-23.061934	2.536742
-71.589303	-20.842924	2.546739
-70.606987	-21.398169	2.556736
-69.902639	-9.644825	2.566733
-69.900360	-15.924924	2.576730
-69.312629	-24.395336	2.586726
-68.886818	-24.728062	2.596723
-68.368969	-16.501195	2.606720
-67.509831	-25.718340	2.616717
-67.083602	-18.047258	2.626714
-66.923031	-27.919836	2.636710
-65.956611	-25.129339	2.646707
-65.511735	-24.286653	2.656704
-65.675537	-20.608438	2.666701
-64.514096	-25.257931	2.676698
-64.026340	-20.966454	2.686694
-64.076443	-31.636622	2.696691
-63.227753	-25.311560	2.706688
-62.491978	-25.642266	2.716685
-62.157273	-31.769565	2.726682
-61.846319	-24.288562	2.736678
-60.941534	-27.491960	2.746675
-60.787239	-24.971110	2.756672
-60.510480	-26.735241	2.766669
-59.392367	-25.466055	2.776666
-59.272060	-22.596156	2.786662
-58.717025	-22.073094	2.796659
-57.877608	-27.871938	2.806656
-57.473705	-29.174509	2.816653
-57.314177	-26.905459	2.826650
-56.821267	-32.947817	2.836646
-56.339009	-30.842271	2.846643
-56.100314	-23.517793	2.856640
-54.874640	-28.840653	2.866637
-54.495611	-27.292319	2.876634
-54.712994	-25.889648	2.886630
-53.480794	-32.772913	2.896627
-52.692480	-20.568420	2.906624
-52.783750	-21.624291	2.916621
-52.498348	-26.234655	2.926618
-51.500922	-17.865225	2.936614
-51.265540	-16.060851	2.946611
-50.830378	-21.221285	2.956608
-50.175891	-26.511830	2.966605
-50.075563	-26.931523	2.976602
-48.828481	-28.177067	2.986598
-48.442206	-17.764993	2.996595
-48.348049	-21.620809	3.006592
-47.943750	-19.013679	3.016589
-46.712228	-21.917517	3.026586
-46.702985	-19.886861	3.036582
-46.405902	-22.996945	3.046579
-45.382400	-16.994343	3.056576
-44.781043	-29.676714	3.066573
-44.928366	-26.698508	3.076570
-44.440067	-31.775105	3.086566
-43.584189	-25.320433	3.096563
-43.318319	-29.407905	3.106560
-42.029611	-23.948088	3.116557
-42.327676	-26.935729	3.126554
-41.817839	-27.545994	3.136550
-41.375750	-24.941589	3.146547
-40.645179	-28.115431	3.156544
-40.348781	-24.097209	3.166541
-39.026926	-26.299822	3.176538
-39.421839	-23.239363	3.186534
-38.579932	-20.835971	3.196531
-38.247858	-29.941195	3.206528
-37.772548	-25.220669	3.216525
-37.281394	-25.959418	3.226522
-36.686083	-32.954350	3.236518
-35.528320	-17.022218	3.246515
-35.149968	-21.097567	3.256512
-35.267038	-16.328559	3.266509
-35.251570	-24.368151	3.276506
-34.002178	-24.791537	3.286502
-33.801466	-24.137654	3.296499
-33.078543	-29.103089	3.306496
-32.292704	-17.479463	3.316493
-32.159025	-20.453320	3.326490
-32.070381	-25.215717	3.336486
-31.422343	-22.223902	3.346483
-30.806751	-27.622379	3.356480
-29.728553	-29.847516	3.366477
-29.819701	-25.350346	3.376474
-29.059533	-18.296097	3.386470
-28.099308	-28.812350	3.396467
-28.010723	-34.121643	3.406464
-27.889775	-31.550003	3.416461
-27.624227	-29.038358	3.426458
-26.625385	-27.387561	3.436454
-26.155742	-15.310676	3.446451
-25.310604	-21.219336	3.456448
-24.828902	-29.006856	3.466445
-24.664828	-25.583294	3.476442
-24.629790	-21.385887	3.486438
-23.696743	-18.824557	3.496435
-23.267960	-27.964430	3.506432
-22.127119	-21.105639	3.516429
-21.774679	-25.846288	3.526426
-21.710189	-28.219450	3.536422
-21.640596	-29.371214	3.546419
-20.483823	-27.129617	3.556416
-20.017263	-26.024780	3.566413
-19.519209	-26.586849	3.576410
-18.577802	-31.534262	3.586406
-18.368764	-26.198855	3.596403
-18.246648	-24.427617	3.606400
-17.917062	-26.506977	3.616397
-16.848309	-19.092849	3.626394
-16.549714	-26.333453	3.636390
-16.447506	-14.862529	3.646387
-15.193339	-23.589528	3.656384
-14.985148	-32.635235	3.666381
-14.624988	-31.142245	3.676378
-14.328360	-29.320981	3.686374
-13.214742	-19.178973	3.696371
-13.149089	-22.350763	3.706368
-12.813395	-26.952294	3.716365
-11.888433	-27.711973	3.726362
-11.608744	-27.401574	3.736358
-11.219631	-15.402978	3.746355
-10.191084	-23.754607	3.756352
-10.010539	-25.121211	3.766349
-10.059236	-23.560260	3.776346
-8.982433	-23.471070	3.786342
-8.528922	-19.815245	3.796339
-8.535307	-21.604230	3.806336
-7.309223	-23.189867	3.816333
-7.036085	-22.535573	3.826330
-6.608691	-19.913308	3.836326
-6.221936	-18.394111	3.846323
-5.752353	-15.413527	3.856320
-4.948223	-12.122231	3.866317
-4.708622	-7.978579	3.876314
-4.359816	-9.396664	3.886310
-3.652444	4.273752	3.896307
-3.562410	14.055411	3.906304
-2.938781	27.013846	3.916301
-2.413647	37.304095	3.926298
-2.084537	46.866433	3.936294
-1.455759	68.661377	3.946291
-1.023648	78.868324	3.956288
-0.494458	86.860820	3.966285
0.018220	111.557283	3.976282
0.000000	124.528328	3.981286
0.559674	133.030424	3.986291
0.721743	133.275535	3.991296
0.678050	138.978522	3.996301
0.888360	139.274420	4.001306
0.644170	163.217017	4.006310
0.914510	158.476681	4.011315
0.859411	175.712507	4.016320
1.157222	173.426563	4.021325
1.486481	167.571172	4.026330
1.219620	169.328895	4.031334
1.217400	178.308815	4.036339
1.565374	172.204632	4.041344
1.263212	173.471142	4.046349
1.346597	171.243730	4.051354
1.463028	173.565263	4.056358
1.660305	178.916229	4.061363
1.675668	175.949075	4.066368
1.377347	179.059810	4.071373
1.206262	166.338316	4.076378
0.956054	170.014107	4.081382
1.123306	168.475654	4.086387
1.347374	185.296669	4.091392
1.407166	175.378385	4.096397
1.613436	180.837573	4.101402
1.304221	186.722252	4.106406
1.417193	176.716194	4.111411
1.543285	181.008266	4.116416
1.399590	179.486765	4.121421
1.469805	166.234003	4.126426
1.441818	181.675917	4.131430
1.637670	169.065109	4.136435
1.476511	182.824009	4.141440
1.347869	178.298181	4.146445
1.583318	171.808169	4.151450
1.577001	181.565078	4.156454
1.293922	185.857476	4.161459
1.301993	186.912188	4.166464
1.707744	176.949226	4.171469
1.616021	175.892686	4.176474
1.580712	180.391552	4.181478
1.620387	168.055738	4.186483
1.711066	174.579211	4.191488
1.614174	187.105548	4.196493
1.745064	183.488514	4.201498
1.429185	187.650796	4.206502
1.367816	168.712841	4.211507
1.419523	183.501561	4.216512
1.446862	185.702928	4.221517
1.739410	196.503790	4.226522
1.864943	214.419441	4.231526
2.335784	207.088722	4.236531
1.811378	200.452283	4.241536
1.752678	188.966733	4.246541
1.601965	185.622057	4.251546
1.981836	183.570914	4.256550
1.832516	177.796250	4.261555
1.355386	187.047313	4.266560
1.605077	202.734950	4.271565
1.784276	205.774214	4.276570
1.981409	213.899127	4.281574
2.201673	195.920922	4.286579
1.985172	204.100374	4.291584
1.715713	200.530147	4.296589
2.249748	192.631662	4.301594
1.659097	199.810268	4.306598
2.103594	195.022228	4.311603
2.044998	194.239604	4.316608
1.800054	196.644886	4.321613
2.054465	199.113984	4.326618
2.013074	201.328751	4.331622
2.139603	201.445387	4.336627
2.366688	194.853353	4.341632
1.794016	193.313959	4.346637
1.692695	177.734727	4.351642
1.787943	200.015266	4.356646
2.026924	200.310543	4.361651
2.191908	216.582960	4.366656
2.268205	210.084458	4.371661
2.293255	214.477989	4.376666
2.075179	226.639504	4.381670
2.248748	212.337272	4.386675
2.282856	210.991244	4.391680
1.702137	205.037464	4.396685
2.322289	206.236909	4.401690
2.066476	221.596753	4.406694
2.318214	221.088343	4.411699
2.027702	219.074820	4.416704
2.171056	210.947039	4.421709
2.146478	209.086255	4.426714
2.209786	216.838155	4.431718
2.553979	202.411471	4.436723
2.085966	219.884894	4.441728
2.019408	210.404159	4.446733
2.108655	215.906294	4.451738
2.192441	225.528671	4.456742
2.063760	213.715124	4.461747
2.139789	214.968900	4.466752
1.892172	220.145977	4.471757
2.278920	221.411254	4.476762
2.125751	218.592674	4.481766
2.278317	215.033598	4.486771
2.225549	217.238024	4.491776
2.011584	238.182365	4.496781
2.573841	241.184804	4.501786
2.269133	242.792143	4.506790
2.447592	249.826754	4.511795
2.111923	254.268413	4.516800
2.222203	251.536278	4.521805
2.449905	241.453685	4.526810
2.110836	242.742122	4.531814
2.195478	236.694115	4.536819
2.542911	239.716868	4.541824
2.277991	240.128462	4.546829
2.861579	238.599933	4.551834
2.589377	242.378655	4.556838
2.748067	228.582476	4.561843
2.828390	237.385319	4.566848
2.518003	246.956602	4.571853
2.840047	233.830446	4.576858
2.497219	247.840218	4.581862
2.677344	237.020799	4.586867
2.542106	250.152271	4.591872
2.466641	234.684124	4.596877
2.729712	228.184367	4.601882
2.761706	239.943996	4.606886
2.526200	240.186322	4.611891
2.427015	245.004848	4.616896
2.367461	236.091649	4.621901
2.926760	240.701860	4.626906
2.659008	241.251663	4.631910
2.656625	232.912281	4.636915
3.023910	249.296739	4.641920
2.635061	250.627392	4.646925
2.917753	244.423919	4.651930
2.790494	256.965425	4.656934
2.771671	238.399982	4.661939
3.026425	243.545662	4.666944
2.560580	243.678274	4.671949
3.044422	249.550151	4.676954
2.862249	257.138436	4.681958
2.924888	254.086054	4.686963
3.079501	246.788341	4.691968
2.600755	244.747495	4.696973
2.969593	243.767135	4.701978
3.107955	268.116948	4.706982
3.326203	250.960319	4.711987
3.175075	247.284178	4.716992
3.166522	250.847399	4.721997
2.873633	247.321509	4.727002
2.868408	250.314672	4.732006
2.789714	242.612727	4.737011
2.768788	240.010344	4.742016
2.709507	242.181125	4.747021
3.469823	256.516273	4.752026
2.710424	256.816275	4.757030
3.127111	249.453689	4.762035
3.389548	254.457989	4.767040
3.182191	258.041429	4.772045
3.195949	254.312424	4.777050
2.979582	245.676292	4.782054
3.006169	235.284757	4.787059
3.387044	247.687134	4.792064
3.090992	256.299565	4.797069
2.916877	239.542448	4.802074
3.402667	262.586569	4.807078
3.363543	255.615871	4.812083
3.016374	244.580788	4.817088
2.907532	260.517516	4.822093
3.313317	255.620254	4.827098
3.285717	273.030797	4.832102
3.443843	272.866703	4.837107
3.456459	267.992558	4.842112
3.169027	256.836241	4.847117
3.340424	259.880759	4.852122
3.232568	272.727879	4.857126
3.447024	252.692974	4.862131
3.440850	263.191491	4.867136
3.194204	263.382586	4.872141
3.439326	261.723438	4.877146
3.413986	266.447211	4.882150
3.139044	265.113277	4.887155
3.098931	266.028990	4.892160
3.186567	266.944781	4.897165
3.842352	269.420782	4.902170
3.485054	266.702821	4.907174
3.329848	280.703539	4.912179
3.323355	267.092452	4.917184
3.261820	265.013632	4.922189
3.675038	263.865659	4.927194
3.376560	267.849443	4.932198
3.519912	276.654856	4.937203
3.662156	266.696760	4.942208
3.268166	269.428353	4.947213
3.488342	266.597635	4.952218
3.373095	266.688351	4.957222
3.399249	269.408915	4.962227
3.350181	269.838702	4.967232
3.359353	280.084066	4.972237
3.498223	269.490324	4.977242
3.595508	275.588671	4.982246
3.776968	272.011163	4.987251
3.501226	270.610664	4.992256
3.285468	273.509966	4.997261
3.624541	280.257809	5.002266
3.629596	293.228851	5.007270
3.910160	298.876028	5.012275
3.626983	281.910255	5.017280
3.145077	291.363258	5.022285
3.970352	290.643089	5.027290
3.781557	306.986244	5.032294
3.844188	301.071914	5.037299
3.999035	299.169456	5.042304
3.760870	308.227741	5.047309
3.887975	303.641804	5.052314
3.798920	301.096714	5.057318
3.804237	305.684768	5.062323
3.885825	302.987981	5.067328
3.997437	313.252649	5.072333
3.864559	295.976533	5.077338
3.555751	293.572558	5.082342
3.884883	299.414126	5.087347
3.906467	308.420950	5.092352
3.776511	304.924599	5.097357
3.769572	316.582421	5.102362
3.751651	303.996775	5.107366
3.695549	300.712321	5.112371
3.973370	296.462852	5.117376
3.715639	312.170018	5.122381
3.862385	302.099065	5.127386
3.656075	302.179461	5.132390
3.801075	309.765882	5.137395
4.086258	303.624922	5.142400
3.833854	307.107722	5.147405
4.007088	303.217220	5.152410
3.959832	298.986460	5.157414
3.780335	312.739446	5.162419
4.299930	311.078676	5.167424
4.027119	316.735154	5.172429
4.082831	318.109729	5.177434
4.543667	314.767767	5.182438
4.126791	311.926105	5.187443
4.170379	309.952746	5.192448
4.286044	310.881444	5.197453
4.225740	295.755853	5.202458
3.993310	307.944090	5.207462
3.994121	295.723365	5.212467
4.325106	318.561433	5.217472
4.034273	314.152705	5.222477
4.244648	317.550102	5.227482
4.489111	330.305953	5.232486
4.076808	322.453203	5.237491
4.294733	323.034369	5.242496
4.379294	332.763244	5.247501
4.322706	322.228003	5.252506
4.346169	323.277995	5.257510
4.311352	314.891271	5.262515
4.382552	322.185872	5.267520
4.091457	321.048993	5.272525
4.339901	331.286786	5.277530
4.285829	329.078450	5.282534
4.463593	331.420202	5.287539
4.577620	335.790493	5.292544
4.479553	346.260532	5.297549
4.592493	336.307263	5.302554
4.599659	336.815716	5.307558
4.328467	320.854315	5.312563
4.674254	309.448656	5.317568
4.175916	316.963425	5.322573
4.452182	322.735842	5.327578
4.366103	322.708835	5.332582
4.333768	332.282499	5.337587
4.457784	329.502483	5.342592
4.671312	324.609529	5.347597
4.738140	335.015054	5.352602
4.891255	346.596764	5.357606
4.676067	323.714598	5.362611
4.426390	306.456503	5.367616
4.605081	316.656744	5.372621
4.938522	316.293210	5.377626
4.785997	313.453391	5.382630
4.482655	307.874775	5.387635
4.801241	306.381407	5.392640
4.617312	308.642772	5.397645
4.620757	297.222194	5.402650
4.511660	302.365618	5.407654
4.484453	305.445919	5.412659
4.794863	325.603078	5.417664
4.632240	345.410672	5.422669
4.888694	324.666970	5.427674
5.007787	329.026945	5.432678
4.630274	316.371212	5.437683
4.657699	325.151718	5.442688
4.506367	339.668664	5.447693
4.632685	330.206314	5.452698
4.877486	338.619175	5.457702
4.701436	334.691606	5.462707
4.961504	331.150550	5.467712
4.910870	340.980047	5.472717
4.944318	335.525016	5.477722
4.892048	328.668162	5.482726
4.457184	335.832579	5.487731
5.185323	329.620153	5.492736
4.870532	337.554741	5.497741
4.871912	327.345725	5.502746
4.867401	340.117905	5.507750
4.876119	342.746660	5.512755
4.926105	332.675194	5.517760
4.710791	335.218048	5.522765
4.757401	333.136044	5.527770
4.713814	327.816563	5.532774
4.597700	330.815346	5.537779
5.095340	333.995884	5.542784
4.838423	338.246481	5.547789
4.619484	335.422236	5.552794
5.019712	354.920206	5.557798
4.970126	359.647840	5.562803
5.427203	362.324818	5.567808
5.521610	363.523652	5.572813
5.291982	353.255531	5.577818
5.031033	346.686140	5.582822
4.684004	335.434098	5.587827
4.860281	347.055964	5.592832
4.834526	362.949783	5.597837
4.889528	362.525771	5.602842
5.187835	364.610295	5.607846
5.300656	372.085470	5.612851
5.063818	373.063093	5.617856
5.141439	369.030600	5.622861
4.912432	369.322168	5.627866
5.192770	379.467272	5.632870
5.317541	371.711907	5.637875
5.527844	361.166812	5.642880
5.013799	367.882838	5.647885
5.218937	369.953643	5.652890
5.415361	372.772220	5.657894
5.312815	376.613154	5.662899
5.155997	363.667913	5.667904
5.364795	363.388638	5.672909
5.439499	361.861011	5.677914
5.466899	377.387648	5.682918
5.302379	374.834567	5.687923
5.553679	361.902399	5.692928
5.290453	367.405355	5.697933
5.293530	373.151369	5.702938
5.526843	372.140642	5.707942
5.462812	377.354745	5.712947
5.664864	362.382818	5.717952
5.329968	365.643527	5.722957
5.352115	362.618377	5.727962
5.378461	364.409872	5.732966
5.280764	364.098660	5.737971
5.590795	369.820096	5.742976
5.473456	374.354754	5.747981
5.390559	365.672493	5.752986
5.693028	381.254647	5.757990
5.530930	379.503132	5.762995
5.612471	377.518720	5.768000
5.496234	388.688599	5.773005
5.752104	378.094083	5.778010
5.621285	381.333702	5.783014
5.589549	401.178220	5.788019
5.601531	387.682752	5.793024
5.753709	393.659146	5.798029
5.592610	381.769556	5.803034
5.448807	379.768332	5.808038
5.338443	388.427918	5.813043
5.747574	372.719245	5.818048
5.681622	390.746258	5.823053
5.819882	391.937410	5.828058
5.741638	399.521712	5.833062
5.396106	395.580265	5.838067
5.489887	393.576056	5.843072
5.444680	385.919189	5.848077
5.758074	392.294833	5.853082
5.927506	386.182946	5.858086
5.553945	386.380929	5.863091
5.734854	386.833667	5.868096
5.359713	393.897213	5.873101
5.850295	405.220607	5.878106
6.170949	419.123016	5.883110
5.855579	405.254514	5.888115
6.212155	399.225773	5.893120
5.837938	393.389149	5.898125
6.096022	382.315921	5.903130
5.945120	397.776705	5.908134
5.661003	394.050211	5.913139
5.863232	393.502664	5.918144
5.772620	422.381149	5.923149
6.252025	410.075457	5.928154
6.077094	422.337897	5.933158
6.194102	411.971865	5.938163
6.134294	391.621637	5.943168
5.932886	399.922807	5.948173
5.667924	391.446224	5.953178
6.238231	401.433625	5.958182
5.826346	409.869636	5.963187
6.080629	410.624141	5.968192
6.083137	422.023344	5.973197
6.449377	425.309214	5.978202
6.095425	419.430534	5.983206
5.943557	422.940458	5.988211
6.095205	411.193238	5.993216
6.160784	421.256257	5.998221
5.982263	415.322568	6.003226
6.073560	412.929426	6.008230
5.817230	419.482066	6.013235
6.063884	417.423436	6.018240
5.971145	412.792509	6.023245
5.817279	419.649183	6.028250
6.054904	418.493681	6.033254
5.814947	423.556874	6.038259
6.054399	423.147195	6.043264
6.279555	418.845272	6.048269
6.028152	420.807065	6.053274
5.936673	414.586979	6.058278
5.931808	420.548441	6.063283
6.331597	404.303548	6.068288
5.945838	435.757209	6.073293
5.981716	416.399233	6.078298
6.138845	419.026422	6.083302
6.011874	412.603258	6.088307
6.063689	415.412133	6.093312
6.050173	425.537832	6.098317
5.804461	435.806325	6.103322
6.120394	438.974857	6.108326
6.216875	449.168722	6.113331
6.389971	440.381116	6.118336
6.165878	429.711038	6.123341
6.211119	428.107196	6.128346
6.209997	417.217728	6.133350
5.937655	424.076337	6.138355
6.170057	414.544798	6.143360
6.022630	424.101931	6.148365
6.138126	427.205305	6.153370
6.372598	423.482198	6.158374
5.742752	430.614735	6.163379
6.237535	425.352554	6.168384
5.885515	429.322782	6.173389
5.994092	425.023066	6.178394
6.558112	443.898168	6.183398
6.167469	447.936390	6.188403
6.148367	422.447038	6.193408
6.143128	430.252668	6.198413
6.067342	426.446151	6.203418
6.436180	426.754779	6.208422
5.949369	421.588461	6.213427
6.505669	417.344769	6.218432
6.244714	427.071933	6.223437
6.303350	416.352503	6.228442
6.150579	420.271061	6.233446
6.000351	429.920621	6.238451
6.098867	428.087698	6.243456
5.921372	430.181854	6.248461
6.152119	415.811124	6.253466
6.243478	421.628916	6.258470
5.883925	431.265120	6.263475
6.040203	422.724226	6.268480
5.978237	433.753494	6.273485
5.867368	425.928733	6.278490
6.130607	428.765815	6.283494
6.082427	420.822695	6.288499
6.190045	430.113266	6.293504
6.074615	438.143037	6.298509
6.230891	431.522613	6.303514
6.585568	422.623731	6.308518
6.045442	430.841503	6.313523
6.074597	429.016556	6.318528
6.213418	428.401600	6.323533
6.452770	426.546255	6.328538
6.353685	426.420373	6.333542
6.101299	433.705072	6.338547
6.186930	432.550757	6.343552
6.215625	434.615378	6.348557
6.011703	428.519749	6.353562
6.134347	428.139549	6.358566
5.855737	423.412823	6.363571
6.145878	420.624519	6.368576
6.101346	438.136926	6.373581
6.234522	424.354286	6.378586
6.320641	420.223672	6.383590
6.015921	421.520030	6.388595
6.543418	420.992025	6.393600
6.219996	427.627058	6.398605
6.507656	429.236401	6.403610
6.561439	419.480972	6.408614
6.359278	428.283120	6.413619
6.294208	410.477797	6.418624
5.994252	402.958774	6.423629
6.006620	405.805778	6.428634
6.341190	409.164594	6.433638
5.757143	418.772786	6.438643
6.475129	407.189947	6.443648
5.974116	402.781595	6.448653
5.999901	410.533119	6.453658
6.191166	409.350592	6.458662
6.445752	415.396604	6.463667
6.288280	398.969847	6.468672
5.927552	393.457176	6.473677
6.033902	404.030228	6.478682
6.214032	391.929795	6.483686
5.908421	394.256784	6.488691
6.183804	409.357432	6.493696
6.519158	412.805315	6.498701
6.085317	404.040465	6.503706
6.274127	396.037247	6.508710
6.059070	391.160846	6.513715
5.911796	395.056580	6.518720
6.026139	399.906362	6.523725
5.897345	398.800715	6.528730
6.390148	400.370628	6.533734
5.893417	407.680931	6.538739
6.021902	407.393495	6.543744
6.118109	423.752155	6.548749
6.413945	421.278640	6.553754
6.426782	417.027401	6.558758
6.224440	400.231782	6.563763
6.026428	396.040655	6.568768
5.997218	398.962058	6.573773
6.100407	399.631168	6.578778
5.918926	388.919699	6.583782
5.639369	405.113663	6.588787
6.021197	410.650709	6.593792
6.126920	425.367535	6.598797
6.319005	427.095180	6.603802
6.334777	418.077594	6.608806
6.219744	426.145182	6.613811
6.415185	419.913320	6.618816
6.330422	407.031053	6.623821
5.970562	400.522085	6.628826
5.848413	389.028778	6.633830
5.886965	408.419394	6.638835
6.368174	411.586102	6.643840
6.318594	416.305070	6.648845
6.081641	415.537674	6.653850
6.186782	403.666963	6.658854
5.963460	413.549283	6.663859
6.029420	413.132920	6.668864
6.210215	415.996924	6.673869
5.997431	425.882434	6.678874
6.288145	416.475983	6.683878
5.907574	414.517463	6.688883
6.378449	416.732167	6.693888
6.476594	408.754667	6.698893
6.344294	402.419024	6.703898
6.324433	392.771758	6.708902
5.718183	397.692175	6.713907
5.906714	393.625256	6.718912
6.008370	400.131213	6.723917
5.818093	407.537199	6.728922
5.999737	411.349061	6.733926
5.986373	420.284994	6.738931
6.157821	428.686021	6.743936
6.547535	430.262614	6.748941
6.259648	422.344338	6.753946
6.161123	415.300955	6.758950
5.889361	411.379211	6.763955
6.074535	417.188709	6.768960
5.998569	424.835200	6.773965
6.354656	416.034558	6.778970
6.404933	417.021293	6.783974
5.983726	413.708503	6.788979
6.331517	398.951487	6.793984
6.006773	408.229845	6.798989
6.049424	400.966851	6.803994
6.230780	399.786367	6.808998
6.225940	396.127907	6.814003
5.850016	398.308123	6.819008
6.037426	409.353546	6.824013
5.965475	421.137694	6.829018
6.302858	434.607934	6.834022
6.018738	430.883010	6.839027
6.144562	432.711062	6.844032
6.133852	427.725500	6.849037
6.037935	433.021094	6.854042
6.396151	423.869427	6.859046
5.999440	429.115756	6.864051
6.096332	429.106091	6.869056
5.865378	423.401933	6.874061
6.345049	421.552229	6.879066
6.241647	411.358600	6.884070
5.981527	423.973828	6.889075
6.300281	421.590831	6.894080
6.081611	413.883452	6.899085
5.999813	425.893809	6.904090
6.439590	416.776345	6.909094
5.869808	415.631118	6.914099
6.151160	422.963654	6.919104
6.208888	424.159709	6.924109
6.247202	419.956331	6.929114
6.132315	410.235258	6.934118
6.162411	404.108437	6.939123
5.948724	397.156429	6.944128
6.396410	409.274720	6.949133
6.015354	403.259061	6.954138
6.162130	397.617042	6.959142
5.828008	395.550557	6.964147
6.138693	407.629062	6.969152
6.324219	422.489108	6.974157
5.934904	414.294652	6.979162
6.303038	423.333531	6.984166
6.377946	418.302561	6.989171
6.050830	403.066305	6.994176
6.292127	401.139402	6.999181
5.973767	408.409401	7.004186
6.245358	393.480152	7.009190
6.287278	402.977384	7.014195
5.925180	403.373363	7.019200
5.992179	398.189398	7.024205
6.142558	400.821652	7.029210
6.252110	395.365002	7.034214
6.003903	406.539265	7.039219
6.036462	403.388055	7.044224
6.176149	399.544546	7.049229
5.693408	410.252616	7.054234
6.157068	411.261416	7.059238
6.401461	424.446167	7.064243
6.570280	416.708125	7.069248
6.351191	402.928407	7.074253
6.092650	405.804060	7.079258
6.385306	403.037442	7.084262
6.282086	399.913537	7.089267
6.160836	398.556414	7.094272
6.271713	398.117785	7.099277
5.594623	400.495470	7.104282
6.079232	394.037952	7.109286
5.763909	404.054355	7.114291
6.019257	400.320482	7.119296
6.087024	405.790339	7.124301
6.004635	402.726118	7.129306
6.193951	397.789410	7.134310
5.821845	408.237748	7.139315
5.958021	416.101761	7.144320
6.384963	421.318733	7.149325
6.117739	420.103483	7.154330
6.510604	415.946749	7.159334
6.300631	408.158204	7.164339
6.124903	399.907731	7.169344
6.257467	402.384091	7.174349
6.106496	400.702357	7.179354
6.154840	397.271071	7.184358
6.155370	403.681751	7.189363
6.027683	394.190343	7.194368
6.314793	393.758338	7.199373
5.822427	394.455198	7.204378
6.139555	400.603092	7.209382
5.914337	402.180264	7.214387
5.979559	392.660740	7.219392
6.094163	402.865178	7.224397
6.194159	403.899692	7.229402
6.187498	398.847753	7.234406
5.933674	412.144114	7.239411
5.871193	403.831403	7.244416
6.362928	421.073107	7.249421
6.122864	428.534542	7.254426
6.356606	414.417090	7.259430
5.986915	411.624004	7.264435
6.344253	408.273571	7.269440
5.906989	402.141158	7.274445
5.968467	412.668196	7.279450
6.339012	408.471168	7.284454
5.986642	416.805135	7.289459
6.046258	408.752738	7.294464
6.336773	426.158727	7.299469
6.361125	425.862551	7.304474
6.294038	405.042277	7.309478
5.925180	404.820733	7.314483
6.104266	405.801450	7.319488
6.324158	408.836753	7.324493
5.995529	400.364038	7.329498
6.360346	396.541719	7.334502
6.381455	408.824449	7.339507
5.907182	397.438997	7.344512
6.446478	403.307440	7.349517
6.105978	408.029372	7.354522
6.372449	393.193329	7.359526
5.933989	407.078242	7.364531
5.943550	407.152160	7.369536
6.060506	401.017022	7.374541
5.801775	408.971731	7.379546
6.183635	402.324678	7.384550
6.168982	402.034393	7.389555
5.985479	395.663850	7.394560
6.459272	389.944588	7.399565
6.192492	403.706242	7.404570
5.994424	390.976417	7.409574
6.078597	398.417886	7.414579
5.943235	398.958714	7.419584
6.160225	395.530970	7.424589
5.766882	400.147229	7.429594
6.363013	397.836928	7.434598
6.119369	401.459585	7.439603
5.987342	390.557360	7.444608
6.170994	394.203122	7.449613
6.122213	399.626834	7.454618
6.243815	392.521614	7.459622
5.861205	397.165689	7.464627
5.889576	397.485913	7.469632
6.187857	412.388382	7.474637
6.145507	429.789120	7.479642
6.500400	424.712598	7.484646
5.779804	412.836256	7.489651
6.027392	413.833215	7.494656
6.071701	428.973474	7.499661
6.264469	430.624045	7.504666
6.368179	422.838608	7.509670
6.225837	409.040010	7.514675
6.265621	403.566734	7.519680
6.352814	409.948213	7.524685
6.110924	412.508323	7.529690
6.091910	399.343206	7.534694
6.124339	403.735564	7.539699
6.120022	399.603806	7.544704
6.495833	399.567515	7.549709
6.263434	404.675819	7.554714
6.121773	400.706603	7.559718
6.178114	395.700039	7.564723
6.281073	394.801357	7.569728
6.203468	397.265288	7.574733
6.098071	408.619072	7.579738
6.014016	391.150423	7.584742
6.258772	398.036343	7.589747
5.588894	395.235928	7.594752
6.252785	396.621115	7.599757
6.133546	392.856165	7.604762
6.204444	388.789658	7.609766
5.763689	396.571360	7.614771
5.865035	398.755327	7.619776
6.254497	394.961669	7.624781
6.061701	398.199556	7.629786
6.098355	391.081224	7.634790
6.273212	397.830364	7.639795
6.216879	399.365652	7.644800
6.400441	393.883282	7.649805
5.949720	399.836158	7.654810
6.030235	387.906207	7.659814
6.092687	397.595779	7.664819
5.870015	398.189994	7.669824
6.170688	399.885182	7.674829
5.958919	399.927808	7.679834
6.290482	396.343872	7.684838
6.121829	399.412576	7.689843
5.502038	407.603913	7.694848
6.301485	413.131931	7.699853
6.317145	416.741290	7.704858
6.461850	401.461935	7.709862
6.109232	390.687149	7.714867
6.306532	396.970203	7.719872
6.171907	401.823479	7.724877
6.150910	399.966615	7.729882
6.007379	395.316508	7.734886
6.199225	400.919268	7.739891
6.166310	406.899002	7.744896
6.178825	394.193374	7.749901
6.210805	399.905783	7.754906
6.373706	399.855941	7.759910
6.320969	399.457138	7.764915
6.367982	405.707749	7.769920
6.410286	388.431619	7.774925
6.212884	403.439754	7.779930
6.205333	392.389359	7.784934
6.242222	389.705116	7.789939
6.057273	392.871446	7.794944
5.762667	392.259662	7.799949
5.839023	396.853104	7.804954
5.945610	390.138540	7.809958
6.039580	383.695241	7.814963
6.030941	389.945033	7.819968
6.394352	394.002356	7.824973
6.087154	398.094973	7.829978
6.242070	390.660586	7.834982
6.381293	401.892009	7.839987
6.148899	406.035342	7.844992
6.361435	399.455112	7.849997
6.143149	407.136498	7.855002
6.231688	410.199752	7.860006
6.065258	408.623990	7.865011
6.001265	411.224783	7.870016
6.523790	403.854992	7.875021
6.083320	417.910352	7.880026
6.442257	399.362243	7.885030
6.215859	406.238268	7.890035
5.931647	408.403242	7.895040
6.526226	405.250970	7.900045
6.144245	395.527137	7.905050
5.710732	388.822227	7.910054
6.206527	386.177150	7.915059
6.340397	398.493819	7.920064
6.202479	385.018532	7.925069
5.813404	385.085892	7.930074
6.127679	387.892382	7.935078
6.417928	392.923480	7.940083
6.225178	393.217310	7.945088
6.251606	377.636969	7.950093
5.876949	376.301050	7.955098
5.875045	377.136220	7.960102
6.239380	392.250285	7.965107
6.150730	401.547215	7.970112
6.282684	384.185937	7.975117
5.941393	383.719653	7.980122
6.398146	385.273322	7.985139
6.279462	386.240921	7.990157
6.051867	386.555425	7.995174
6.393075	377.604200	8.000192
6.075982	379.394072	8.005210
6.245009	380.270940	8.010227
6.003435	376.916459	8.015245
6.068120	381.688455	8.020262
6.353545	373.148239	8.025280
6.025198	382.431992	8.030298
6.167739	380.429872	8.035315
6.185559	378.153628	8.040333
5.823902	383.427943	8.045350
6.172158	381.001115	8.050368
5.899367	396.589618	8.055386
6.116000	397.020228	8.060403
6.729592	405.787230	8.065421
6.163010	388.940387	8.070438
6.096228	392.510140	8.075456
6.247145	395.020378	8.080474
6.348943	400.907760	8.085491
6.114118	386.051454	8.090509
6.084160	394.359327	8.095526
6.482484	390.623707	8.100544
6.325635	402.901717	8.105562
6.094013	399.124160	8.110579
6.483579	398.463134	8.115597
6.061590	390.012736	8.120614
6.263929	392.030024	8.125632
6.320726	394.415368	8.130650
6.203408	391.719696	8.135667
6.548512	399.487127	8.140685
6.709418	395.465210	8.145702
6.108457	381.644281	8.150720
6.177914	373.133072	8.155738
6.070327	373.215641	8.160755
6.411127	384.317127	8.165773
6.333311	390.267426	8.170790
6.694818	387.199676	8.175808
6.425665	386.442448	8.180826
6.028156	380.407249	8.185843
6.596680	380.358150	8.190861
6.020811	378.540000	8.195878
6.336716	383.713505	8.200896
6.333796	388.010958	8.205914
6.563194	384.075092	8.210931
6.485030	374.623549	8.215949
6.184166	368.709680	8.220966
6.296279	364.383312	8.225984
6.146760	375.749933	8.231002
5.856118	387.482309	8.236019
6.330151	385.003869	8.241037
5.981438	394.242004	8.246054
6.362696	391.513260	8.251072
6.355916	388.915543	8.256090
6.398500	391.810879	8.261107
6.521667	389.532673	8.266125
6.167914	398.441757	8.271142
6.664515	398.728008	8.276160
6.546968	400.838423	8.281178
6.220453	402.249584	8.286195
6.556077	390.608584	8.291213
6.400871	406.767656	8.296230
6.868846	403.594418	8.301248
6.517106	399.256368	8.306266
6.300869	396.062027	8.311283
6.678971	393.974102	8.316301
6.372452	397.583899	8.321318
6.532535	396.401816	8.326336
6.521627	407.067334	8.331354
6.466165	394.121777	8.336371
6.842718	381.319759	8.341389
6.380194	395.735973	8.346406
6.449252	391.332510	8.351424
6.474748	399.091455	8.356442
6.151047	397.512269	8.361459
6.676653	389.533444	8.366477
6.073947	390.463592	8.371494
6.296960	395.882834	8.376512
6.176790	402.287381	8.381530
6.390791	401.289034	8.386547
6.457897	396.658159	8.391565
5.945833	399.478379	8.396582
6.318634	413.705576	8.401600
6.611917	420.659266	8.406618
6.603753	424.618261	8.411635
7.068416	419.773479	8.416653
6.548515	429.049339	8.421670
6.754273	424.292861	8.426688
6.557705	401.810012	8.431706
6.464419	402.525578	8.436723
6.892338	409.067944	8.441741
6.552694	397.873005	8.446758
6.407072	403.015364	8.451776
6.545917	409.481184	8.456794
6.816710	422.793146	8.461811
7.002881	408.208939	8.466829
6.606779	408.004848	8.471846
6.699222	397.480936	8.476864
6.728540	398.174943	8.481882
6.331631	399.830657	8.486899
6.831298	395.153276	8.491917
6.407455	400.661534	8.496934
6.664337	400.961648	8.501952
6.498269	416.055704	8.506970
6.618836	424.727712	8.511987
6.706323	422.669388	8.517005
6.593815	419.693606	8.522022
6.736523	429.545096	8.527040
6.769469	425.378708	8.532058
6.602505	432.273678	8.537075
6.786710	434.367994	8.542093
6.726263	432.479914	8.547110
6.743549	429.100307	8.552128
7.028488	425.121738	8.557146
6.878291	418.399216	8.562163
6.939106	398.449931	8.567181
6.558206	415.992856	8.572199
6.411937	401.090324	8.577216
6.694607	412.336125	8.582234
6.939129	432.317992	8.587251
7.153434	430.224220	8.592269
6.756224	423.415206	8.597287
6.620512	407.171468	8.602304
6.526144	410.801907	8.607322
6.928152	427.610048	8.612339
6.981751	419.231950	8.617357
6.523774	422.614785	8.622375
6.791966	429.354558	8.627392
7.057078	432.158786	8.632410
7.006098	429.307212	8.637427
6.812277	407.122297	8.642445
6.491191	410.500879	8.647463
6.637290	428.594748	8.652480
6.996788	427.296848	8.657498
6.638803	438.475743	8.662515
6.723012	426.090357	8.667533
6.896764	438.288447	8.672551
7.004142	429.031011	8.677568
7.157104	422.072683	8.682586
6.788724	420.962885	8.687603
6.901010	428.164556	8.692621
6.960080	427.743484	8.697639
7.050069	425.399730	8.702656
6.958896	427.693150	8.707674
6.484422	443.009540	8.712691
7.011336	439.421811	8.717709
6.903342	434.705275	8.722727
6.694780	434.854821	8.727744
6.803414	429.110244	8.732762
6.545687	431.750413	8.737779
6.635949	430.902738	8.742797
6.952079	424.585337	8.747815
7.047491	435.051723	8.752832
7.025435	425.652432	8.757850
7.042099	441.694792	8.762867
7.018578	427.505230	8.767885
7.013827	429.480375	8.772903
6.695735	426.090969	8.777920
6.768743	432.271901	8.782938
6.823373	441.445582	8.787955
6.709267	429.741128	8.792973
6.964517	430.602880	8.797991
6.720488	434.789254	8.803008
7.159407	435.177801	8.808026
7.195824	439.451802	8.813043
7.230907	427.268657	8.818061
7.063047	436.794247	8.823079
7.040979	444.616628	8.828096
6.943013	424.387232	8.833114
6.904595	432.769163	8.838131
6.838290	428.607067	8.843149
7.144408	445.105997	8.848167
7.048624	456.615701	8.853184
7.490016	441.153289	8.858202
7.384513	443.811068	8.863219
7.252027	437.972325	8.868237
7.254716	436.638660	8.873255
7.232800	436.266085	8.878272
7.394309	428.464480	8.883290
7.581548	439.342930	8.888307
7.181061	433.994166	8.893325
7.288147	442.064543	8.898343
7.383251	433.562816	8.903360
7.450234	427.207109	8.908378
7.296637	433.918772	8.913395
6.683543	427.965840	8.918413
6.908490	429.499891	8.923431
6.679449	443.474622	8.928448
6.836062	436.080287	8.933466
6.610484	444.171511	8.938483
6.756931	430.198359	8.943501
7.012954	437.852084	8.948519
7.160870	449.689156	8.953536
7.637672	450.985105	8.958554
7.392092	446.051889	8.963571
7.282972	442.084290	8.968589
7.021257	438.340857	8.973607
6.828912	442.273585	8.978624
7.057741	443.978827	8.983642
7.435871	459.692449	8.988659
7.078544	462.226550	8.993677
7.250315	463.725352	8.998695
7.181888	471.061795	9.003712
7.348435	456.581582	9.008730
7.112212	464.869845	9.013747
7.344179	472.335280	9.018765
7.426022	459.394797	9.023783
7.223844	471.216657	9.028800
7.161424	458.936514	9.033818
7.033411	473.081865	9.038835
7.229836	462.395362	9.043853
7.599309	456.181475	9.048871
7.582034	454.830065	9.053888
7.592082	462.099921	9.058906
7.326400	454.171295	9.063923
7.112398	445.994930	9.068941
7.312794	441.718035	9.073959
7.573494	467.137714	9.078976
7.482145	453.130254	9.083994
7.539373	445.306214	9.089011
7.021931	437.155489	9.094029
7.345825	444.244640	9.099047
7.145089	462.165116	9.104064
7.419041	467.507025	9.109082
7.678729	468.016695	9.114099
7.154012	465.471197	9.119117
7.545318	459.309974	9.124135
7.418254	463.096436	9.129152
7.420496	463.077294	9.134170
7.614087	468.792568	9.139187
7.243567	454.040240	9.144205
7.794356	460.159682	9.149223
7.262382	456.183237	9.154240
7.406676	441.649852	9.159258
7.577915	454.469380	9.164275
7.623959	447.660886	9.169293
7.767879	449.306233	9.174311
7.424423	438.787231	9.179328
7.149990	433.603523	9.184346
7.129243	435.601995	9.189363
7.319296	455.278604	9.194381
7.683274	453.885280	9.199399
7.398843	465.761946	9.204416
7.606021	462.361202	9.209434
7.259686	464.169132	9.214451
7.439527	463.636852	9.219469
7.826922	464.039279	9.224487
7.365573	471.573695	9.229504
7.482627	465.178944	9.234522
7.467725	472.656871	9.239539
7.628557	470.023408	9.244557
7.806557	459.537788	9.249575
7.385602	466.402161	9.254592
7.432647	461.899787	9.259610
7.330039	455.075450	9.264627
7.667702	461.374989	9.269645
7.803216	468.427752	9.274663
7.264696	468.954750	9.279680
7.148855	463.383483	9.284698
7.248663	465.914432	9.289715
6.937546	479.037756	9.294733
7.397212	474.117023	9.299751
7.774274	504.512654	9.304768
7.867262	497.305424	9.309786
7.782542	488.228688	9.314803
7.661361	486.604611	9.319821
7.914975	470.830891	9.324839
7.633763	475.917866	9.329856
7.796548	471.281301	9.334874
7.861533	468.590154	9.339891
7.692186	479.412950	9.344909
8.074816	468.875990	9.349927
7.863853	467.882334	9.354944
7.655028	469.703232	9.359962
7.574468	461.012401	9.364979
7.401033	463.373824	9.369997
7.417180	455.030276	9.375015
7.571548	468.563186	9.380032
7.551722	467.252944	9.385050
7.550964	481.337784	9.390067
7.951394	494.806395	9.395085
7.912507	494.340585	9.400103
7.660522	493.057905	9.405120
8.040240	493.303749	9.410138
7.741422	478.551486	9.415155
7.458168	480.997892	9.420173
7.661071	485.348359	9.425191
7.928878	490.124812	9.430208
8.038403	496.731159	9.435226
7.845698	502.162849	9.440243
7.683703	489.739797	9.445261
8.026896	485.750545	9.450279
7.760653	488.865916	9.455296
7.612512	492.726946	9.460314
8.322600	492.609440	9.465331
7.961400	493.044569	9.470349
7.539903	477.471827	9.475367
7.852714	482.876371	9.480384
8.042020	486.801183	9.485402
7.947465	470.005114	9.490419
7.508520	470.991897	9.495437
7.798199	481.815951	9.500455
8.165446	493.949643	9.505472
8.013667	494.720208	9.510490
8.156738	484.270689	9.515507
7.651706	480.253541	9.520525
8.014790	470.657936	9.525543
7.894209	486.284609	9.530560
8.003376	485.786317	9.535578
7.740549	480.221170	9.540595
7.251631	495.756726	9.545613
7.568920	492.464632	9.550631
7.830803	492.835170	9.555648
7.986707	502.765412	9.560666
8.098688	505.968301	9.565683
8.025635	494.188280	9.570701
8.577544	496.384072	9.575719
8.323254	499.865340	9.580736
8.179460	491.723538	9.585754
8.054544	504.042576	9.590771
7.972162	496.520431	9.595789
8.195230	495.486716	9.600807
8.148314	496.035145	9.605824
7.876504	502.806246	9.610842
8.150214	501.824541	9.615859
7.754489	499.453054	9.620877
8.065554	499.220193	9.625895
7.721687	493.146312	9.630912
7.932946	509.687651	9.635930
8.130552	504.860265	9.640947
8.045742	513.759553	9.645965
8.033178	503.677592	9.650983
7.889426	501.206157	9.656000
7.848831	501.736214	9.661018
7.974122	497.198188	9.666035
7.983159	508.549181	9.671053
8.384310	507.545113	9.676071
8.040511	500.092792	9.681088
8.150598	504.254181	9.686106
8.240879	503.698010	9.691123
8.020355	503.491110	9.696141
7.828499	498.078712	9.701159
7.993781	500.809789	9.706176
7.882139	507.672174	9.711194
8.557904	509.542290	9.716211
8.144028	520.334111	9.721229
7.939128	507.604620	9.726247
7.980144	519.884281	9.731264
7.940573	531.607316	9.736282
8.243966	538.219446	9.741299
8.294041	534.225757	9.746317
8.062164	528.917236	9.751335
8.729386	530.988561	9.756352
8.283838	533.056275	9.761370
8.673089	519.499143	9.766387
8.102602	525.127087	9.771405
8.319467	516.925718	9.776423
8.400522	512.188956	9.781440
8.547962	525.068399	9.786458
8.339268	506.617387	9.791475
8.044248	500.765483	9.796493
8.352292	510.526950	9.801511
8.436558	496.782756	9.806528
8.153301	506.241356	9.811546
8.289749	503.596587	9.816563
8.105809	514.544854	9.821581
8.259043	531.388749	9.826599
8.615388	528.182077	9.831616
8.344570	531.218696	9.836634
8.427831	525.369059	9.841651
8.114869	528.223525	9.846669
8.300897	529.468214	9.851687
8.384319	533.252186	9.856704
8.282121	530.902962	9.861722
8.558163	531.485893	9.866739
8.108294	535.642537	9.871757
8.269071	531.181076	9.876775
8.673327	520.694419	9.881792
8.264093	529.230352	9.886810
8.171813	526.827910	9.891827
8.109937	526.786553	9.896845
8.376678	525.213339	9.901863
8.155000	524.205714	9.906880
7.965433	529.663267	9.911898
8.439469	529.737149	9.916915
8.628878	552.304099	9.921933
8.857911	541.278095	9.926951
8.593214	543.005148	9.931968
8.164574	528.058489	9.936986
8.284756	526.163207	9.942003
8.629522	537.315517	9.947021
8.803278	544.093871	9.952039
9.048817	522.396739	9.957056
8.421971	529.306385	9.962074
8.880212	522.408481	9.967091
8.759061	529.660022	9.972109
8.552875	519.515360	9.977127
8.514696	534.225116	9.982144
8.714909	532.776532	9.987162
8.621407	521.712427	9.992179
8.463344	533.596484	9.997197
8.473541	526.941146	10.002215
8.746861	517.312798	10.007232
8.446845	534.959136	10.012250
8.564987	528.190981	10.017267
8.654094	533.236696	10.022285
8.242958	533.503961	10.027303
8.712887	521.323458	10.032320
8.220552	529.923593	10.037338
8.778698	540.830614	10.042355
8.733020	553.204036	10.047373
8.759812	550.396791	10.052391
8.325368	547.746519	10.057408
8.325725	566.832804	10.062426
8.171506	554.414313	10.067443
8.381318	565.820748	10.072461
8.527655	566.989957	10.077479
8.844977	560.146166	10.082496
8.585546	565.364381	10.087514
8.698205	561.487437	10.092531
8.780785	559.218905	10.097549
8.809072	557.013724	10.102567
8.916945	550.194515	10.107584
8.727271	560.591451	10.112602
8.670950	555.954865	10.117619
9.078340	564.616086	10.122637
8.806737	563.106366	10.127655
9.141677	564.933343	10.132672
8.769099	565.719352	10.137690
9.167721	561.859439	10.142707
9.032986	561.337517	10.147725
8.826977	556.340015	10.152743
8.975178	564.243399	10.157760
9.196873	563.382138	10.162778
9.152298	562.613161	10.167795
9.217696	558.978110	10.172813
8.800331	553.070936	10.177831
8.749543	526.987986	10.182848
8.771752	543.233056	10.187866
8.712028	558.408385	10.192883
8.991587	553.345727	10.197901
8.596763	566.491699	10.202919
9.168095	554.553350	10.207936
8.712911	556.245929	10.212954
8.764254	561.481576	10.217971
9.104853	556.009592	10.222989
8.613605	560.731341	10.228007
9.160657	555.951951	10.233024
9.015766	558.392889	10.238042
8.936717	556.331916	10.243059
9.049496	554.824050	10.248077
8.429458	563.524556	10.253095
8.453691	557.584923	10.258112
8.872577	561.571783	10.263130
8.876625	570.285875	10.268147
9.045910	562.492753	10.273165
8.732054	567.017710	10.278183
8.673119	571.758150	10.283200
8.732215	584.999149	10.288218
9.193626	579.036248	10.293235
9.506595	581.338494	10.298253
9.134538	588.660110	10.303271
9.482342	586.291590	10.308288
9.378084	572.725895	10.313306
9.142212	570.602017	10.318323
9.123178	566.180866	10.323341
8.825127	575.113664	10.328359
9.057749	553.553074	10.333376
8.823303	566.473192	10.338394
9.007580	575.470298	10.343411
9.333647	596.159041	10.348429
9.115948	597.086421	10.353447
9.048130	584.382110	10.358464
9.199798	584.483788	10.363482
9.075168	591.270619	10.368499
9.359863	587.028488	10.373517
9.152720	588.528476	10.378535
9.536935	585.471675	10.383552
9.314475	577.682246	10.388570
8.990807	563.301719	10.393587
9.101168	577.244565	10.398605
9.337482	588.959186	10.403623
8.917908	589.264858	10.408640
8.979559	586.528972	10.413658
9.132961	598.340052	10.418675
9.875619	586.479493	10.423693
9.456418	598.324924	10.428711
9.625973	583.433102	10.433728
9.154890	575.760779	10.438746
9.060111	559.939176	10.443763
9.203061	571.657886	10.448781
9.330820	586.321214	10.453799
9.279363	588.014797	10.458816
9.529174	593.935914	10.463834
9.336512	586.875720	10.468851
9.245890	587.375908	10.473869
9.012393	586.752299	10.478887
9.305311	581.519906	10.483904
9.339265	581.243150	10.488922
9.177808	592.534952	10.493939
9.296296	585.243135	10.498957
8.917229	594.904510	10.503975
9.107704	587.501325	10.508992
9.579842	596.508466	10.514010
9.535637	596.453346	10.519027
9.792774	590.956839	10.524045
9.456011	595.459826	10.529063
9.797915	598.208411	10.534080
9.548918	593.986682	10.539098
9.396352	595.947248	10.544115
9.532284	588.350388	10.549133
9.502004	584.720801	10.554151
9.825832	590.005452	10.559168
9.848578	583.770804	10.564186
9.793755	593.113148	10.569203
9.896034	581.707823	10.574221
9.388609	583.219142	10.579239
9.272604	565.468541	10.584256
9.576968	572.524976	10.589274
9.274825	580.647106	10.594291
9.477961	588.471298	10.599309
9.498335	595.070066	10.604327
9.400175	590.743155	10.609344
9.829144	594.111075	10.614362
9.692877	598.776786	10.619379
9.656878	595.209953	10.624397
9.811886	589.295614	10.629415
9.920088	597.907772	10.634432
9.507804	576.016188	10.639450
9.419107	572.962212	10.644467
9.616338	583.998539	10.649485
9.230995	588.193876	10.654503
9.471627	588.587829	10.659520
9.411101	589.048767	10.664538
9.426922	594.898549	10.669555
9.410195	590.806114	10.674573
9.110556	595.453116	10.679591
9.308799	587.432154	10.684608
9.699962	606.345076	10.689626
9.776456	626.043336	10.694643
9.879125	614.683193	10.699661
9.573637	620.545842	10.704679
9.622913	622.540770	10.709696
9.825442	615.673322	10.714714
10.003230	626.540090	10.719731
9.950610	610.878540	10.724749
9.679929	603.191200	10.729767
9.667909	594.832771	10.734784
9.675392	604.078159	10.739802
9.909713	618.176999	10.744819
9.946477	623.837105	10.749837
9.732642	602.341599	10.754855
9.571157	603.161023	10.759872
10.097261	614.832614	10.764890
9.710677	631.737605	10.769907
10.046912	617.906151	10.774925
10.047238	630.349540	10.779943
9.936657	610.750491	10.784960
9.996662	595.216880	10.789978
9.811429	587.731863	10.794995
10.107000	581.032415	10.800013
9.918875	587.487306	10.805031
9.741987	597.625469	10.810048
9.940539	577.031260	10.815066
9.794264	588.257154	10.820083
10.044863	588.206966	10.825101
9.721816	599.963391	10.830119
9.532670	612.108954	10.835136
10.051739	615.003671	10.840154
9.687041	623.281288	10.845171
9.764744	622.349870	10.850189
9.915568	625.961257	10.855207
10.105571	625.329849	10.860224
10.356427	624.252534	10.865242
10.262186	623.864025	10.870259
10.335512	617.457386	10.875277
9.973560	623.486299	10.880295
10.064941	627.636265	10.885312
10.640666	611.917122	10.890330
10.051951	611.701345	10.895347
10.123757	587.207240	10.900365
10.015752	593.016583	10.905383
9.623309	589.170442	10.910400
10.268984	610.197781	10.915418
10.004489	620.853631	10.920435
10.135338	615.224576	10.925453
10.087582	618.638670	10.930471
9.836748	616.880630	10.935488
9.961167	619.081948	10.940506
9.807316	619.167878	10.945523
9.956385	623.208655	10.950541
9.985756	623.184413	10.955559
10.068739	620.942377	10.960576
10.394978	616.840959	10.965594
9.573769	626.396132	10.970611
9.857514	618.815041	10.975629
10.245408	629.620710	10.980647
10.405390	644.846016	10.985664
10.489887	643.815838	10.990682
10.258290	637.442551	10.995699
10.294757	619.657491	11.000717
10.152444	609.907239	11.005735
10.115309	628.450466	11.010752
10.389204	632.610055	11.015770
10.546345	644.812644	11.020787
10.559328	631.705326	11.025805
10.323134	618.916186	11.030823
9.988795	624.841895	11.035840
10.533634	623.103954	11.040858
10.371348	626.728213	11.045875
10.427441	622.537059	11.050893
10.268046	619.233428	11.055911
10.310467	624.924482	11.060928
10.473319	616.366713	11.065946
10.607060	625.152974	11.070963
10.258835	617.390923	11.075981
10.329268	613.137354	11.080999
10.312053	619.341428	11.086016
10.420999	612.808407	11.091034
10.599754	637.184197	11.096051
10.274736	619.748370	11.101069
10.476289	629.653194	11.106087
10.465778	638.444149	11.111104
10.669130	633.197493	11.116122
10.467372	635.138486	11.121139
10.548390	623.449284	11.126157
10.663979	624.693091	11.131175
10.311488	628.810937	11.136192
10.914888	617.677580	11.141210
10.709149	618.003218	11.146227
10.490911	616.875733	11.151245
10.721930	618.775497	11.156263
10.451076	615.170733	11.161280
10.598826	617.705942	11.166298
10.266775	617.298106	11.171315
10.018782	623.341736	11.176333
10.323828	629.048978	11.181351
10.678873	650.758094	11.186368
10.668642	639.689512	11.191386
10.674503	646.612146	11.196403
10.645391	650.452250	11.201421
10.386839	634.898915	11.206439
10.653349	652.797850	11.211456
10.899445	644.278588	11.216474
10.896403	651.628262	11.221491
10.868540	641.787516	11.226509
11.028667	652.332459	11.231527
10.411710	639.150325	11.236544
11.128498	638.138862	11.241562
10.739674	628.804345	11.246579
10.495271	616.665339	11.251597
10.579568	627.407500	11.256615
10.952536	646.174294	11.261632
10.883953	631.123992	11.266650
10.570107	627.345479	11.271667
10.662929	632.817545	11.276685
10.771428	639.386725	11.281703
10.867338	640.817451	11.286720
10.777821	639.962641	11.291738
11.009244	653.356144	11.296755
11.140241	651.645846	11.301773
11.152050	634.902583	11.306791
10.793105	629.681284	11.311808
10.999886	622.744233	11.316826
11.193785	623.857908	11.321843
10.795320	624.034097	11.326861
10.988956	616.624862	11.331879
10.806225	628.285747	11.336896
10.743552	615.112679	11.341914
10.696642	617.881211	11.346931
10.669293	622.235344	11.351949
10.944437	629.284065	11.356967
11.121428	638.810527	11.361984
10.694931	627.297403	11.367002
10.656127	636.262140	11.372019
10.835279	644.108258	11.377037
11.143263	645.047275	11.382055
10.831155	649.785335	11.387072
10.994463	644.996281	11.392090
11.137023	649.024763	11.397107
11.112335	648.709725	11.402125
11.082627	636.883220	11.407143
11.259191	646.102302	11.412160
11.134757	645.898718	11.417178
11.130748	650.253507	11.422195
10.719853	654.609002	11.427213
10.905554	648.388185	11.432231
10.641375	647.733652	11.437248
10.839778	651.897527	11.442266
10.908052	652.827571	11.447283
10.951913	648.372716	11.452301
11.437868	645.372610	11.457319
11.115604	642.559394	11.462336
11.104075	647.794499	11.467354
11.253502	638.550223	11.472371
11.067236	640.593948	11.477389
11.270294	650.449524	11.482407
11.273203	644.641541	11.487424
11.039549	653.171387	11.492442
11.410346	651.972568	11.497459
11.015348	646.256901	11.502477
11.137301	644.550272	11.507495
11.047584	647.183613	11.512512
11.130401	642.326645	11.517530
10.914957	643.655788	11.522547
11.108854	662.932054	11.527565
11.247486	667.495405	11.532583
11.127389	664.864315	11.537600
11.182961	684.720052	11.542618
11.142363	675.376640	11.547635
11.143404	681.319652	11.552653
11.671080	673.093311	11.557671
11.706429	673.889470	11.562688
11.536129	685.512312	11.567706
11.734561	671.474794	11.572723
11.403488	676.908876	11.577741
11.631599	654.860152	11.582759
11.407642	657.618161	11.587776
11.407210	652.411669	11.592794
11.321090	646.089390	11.597811
11.351753	650.800200	11.602829
11.078567	655.505416	11.607847
11.117969	669.277082	11.612864
11.575098	679.367985	11.617882
11.565806	672.929389	11.622899
11.660361	673.866484	11.627917
11.942861	675.187269	11.632935
11.514360	672.442489	11.637952
11.472912	661.519031	11.642970
11.563558	664.872339	11.647987
11.582734	676.472932	11.653005
11.196309	672.105138	11.658023
11.515918	673.910663	11.663040
11.379688	678.198073	11.668058
11.557305	676.582575	11.673075
11.322012	688.232165	11.678093
11.379324	679.326774	11.683111
11.559186	682.593215	11.688128
11.409577	673.698599	11.693146
11.517537	675.034026	11.698163
10.986726	679.792502	11.703181
11.436453	679.114970	11.708199
11.663732	681.904077	11.713216
11.542089	683.526271	11.718234
11.542382	680.088416	11.723251
11.338641	703.191567	11.728269
11.823936	701.194045	11.733287
11.993888	707.688084	11.738304
12.063773	699.804729	11.743322
11.621264	693.751297	11.748339
11.724219	703.944191	11.753357
11.959981	699.932980	11.758375
12.161408	680.402251	11.763392
11.827565	684.616217	11.768410
11.706822	673.404771	11.773427
11.339813	675.301784	11.778445
11.943482	678.421804	11.783463
12.187116	673.317445	11.788480
11.880201	670.184571	11.793498
12.058714	677.406647	11.798515
11.654490	679.295871	11.803533
11.973313	670.505077	11.808551
11.870558	662.306367	11.813568
11.426241	679.064915	11.818586
12.064168	666.599505	11.823603
11.779659	679.220188	11.828621
11.583872	683.901526	11.833639
11.873425	698.430990	11.838656
12.121162	709.411180	11.843674
12.159155	710.343112	11.848691
11.990891	703.269755	11.853709
11.971688	695.600014	11.858727
12.026183	690.007636	11.863744
11.897577	687.840717	11.868762
12.190093	697.244478	11.873779
12.162881	684.504597	11.878797
12.009909	684.847842	11.883815
12.026923	686.342273	11.888832
11.868575	688.140240	11.893850
12.133413	687.547962	11.898867
11.967660	700.884499	11.903885
12.306076	704.144275	11.908903
12.152478	689.186782	11.913920
12.021221	688.171203	11.918938
12.260535	692.160584	11.923955
11.853318	695.397846	11.928973
12.342818	704.555697	11.933991
11.940981	696.773582	11.939008
11.991546	713.385349	11.944026
12.555374	709.328859	11.949043
12.363673	710.365106	11.954061
12.111306	699.774687	11.959079
12.193237	694.667475	11.964096
11.851848	721.466490	11.969114
12.422138	710.804285	11.974131
12.388072	720.556612	11.979149
12.255334	709.357369	11.984167
12.359342	703.936665	11.989184
12.235681	718.172847	11.994202
12.535312	709.150790	11.999219
12.406741	688.133477	12.004237
12.088865	689.500316	12.009255
12.600062	689.360558	12.014272
12.431469	686.608991	12.019290
12.034704	681.655949	12.024307
12.096024	675.599288	12.029325
12.312483	688.093998	12.034343
12.485521	701.062042	12.039360
12.467427	715.606439	12.044378
12.537844	688.121480	12.049395
12.346174	708.864934	12.054413
12.005775	711.541133	12.059431
12.454946	700.558343	12.064448
12.237222	701.836298	12.069466
12.219757	701.091350	12.074483
12.127899	711.745338	12.079501
12.276488	705.684789	12.084519
12.622952	703.761520	12.089536
12.508459	711.116362	12.094554
12.418806	705.367636	12.099571
12.563200	714.264766	12.104589
12.295693	704.310476	12.109607
12.283335	707.296100	12.114624
12.549978	702.695940	12.119642
12.456524	707.803944	12.124659
12.530022	706.234881	12.129677
12.331259	699.174074	12.134695
12.558627	698.324658	12.139712
12.432372	719.041309	12.144730
12.891741	721.920972	12.149747
12.671641	718.194763	12.154765
12.589535	705.471075	12.159783
12.493505	710.020690	12.164800
12.782200	729.676530	12.169818
12.763956	724.376918	12.174835
12.831274	714.966926	12.179853
12.536943	719.210552	12.184871
12.756627	719.809552	12.189888
12.796216	723.101285	12.194906
13.033982	715.420514	12.199923
12.951463	707.145390	12.204941
12.491823	717.805004	12.209959
12.538239	694.823107	12.214976
12.629791	718.470463	12.219994
12.759987	716.382957	12.225011
13.018056	726.367420	12.230029
12.869969	733.962485	12.235047
13.216856	723.117143	12.240064
12.702837	715.488300	12.245082
12.559380	705.237427	12.250099
13.080369	730.408583	12.255117
12.973875	720.863316	12.260135
12.881450	701.791214	12.265152
12.839798	710.292722	12.270170
13.002474	709.013145	12.275187
13.036489	716.609231	12.280205
12.925356	709.952722	12.285223
12.983545	713.101214	12.290240
12.957921	711.654130	12.295258
13.143785	712.200487	12.300275
13.094561	702.863215	12.305293
12.885852	705.135072	12.310311
12.879949	697.066889	12.315328
12.751093	714.713721	12.320346
12.906794	725.277755	12.325363
13.241404	725.068339	12.330381
13.011473	734.961884	12.335399
13.171294	732.274415	12.340416
12.883633	735.650463	12.345434
12.877485	738.149268	12.350451
13.085384	731.434605	12.355469
12.795322	728.889821	12.360487
12.895089	735.310307	12.365504
12.993083	749.515975	12.370522
12.933855	733.989642	12.375539
13.044172	727.612634	12.380557
13.021403	732.672286	12.385575
13.035034	728.141335	12.390592
13.208578	727.283148	12.395610
13.221160	730.395133	12.400627
13.519424	729.500469	12.405645
13.143553	726.339481	12.410663
13.224460	725.334301	12.415680
13.112445	731.482922	12.420698
13.438894	733.125911	12.425715
13.238434	730.228069	12.430733
13.030270	734.223536	12.435751
13.204627	733.088067	12.440768
13.411720	729.824868	12.445786
13.319975	745.406068	12.450803
13.752221	730.123815	12.455821
13.439293	747.885328	12.460839
13.654095	725.933788	12.465856
13.506697	732.166237	12.470874
13.571418	728.604678	12.475891
13.746923	726.049239	12.480909
13.565694	724.917366	12.485927
13.715284	724.351132	12.490944
13.752202	731.690265	12.495962
13.312070	732.225127	12.500979
13.448619	724.653885	12.505997
13.441737	719.661419	12.511015
13.751843	713.887778	12.516032
13.363599	722.464024	12.521050
13.039743	720.781883	12.526067
13.426495	725.044975	12.531085
13.282421	735.163208	12.536103
13.493660	720.839680	12.541120
13.618119	720.754360	12.546138
13.357667	722.409865	12.551155
13.576769	722.617650	12.556173
13.266581	719.980550	12.561191
13.308171	716.418115	12.566208
13.559958	730.823384	12.571226
13.929853	742.468875	12.576243
14.136588	732.740249	12.581261
13.684144	722.933999	12.586279
13.376259	721.267313	12.591296
13.607992	722.727633	12.596314
13.776271	738.767540	12.601331
13.729737	725.990879	12.606349
13.910411	732.490823	12.611367
13.788414	732.097673	12.616384
13.818783	724.508845	12.621402
13.624137	726.819506	12.626419
13.854988	722.607546	12.631437
13.488430	726.681892	12.636455
14.023594	740.573962	12.641472
13.895995	739.748703	12.646490
13.952152	745.975669	12.651507
14.113853	730.246095	12.656525
13.785896	726.173270	12.661543
14.188243	719.553843	12.666560
13.913773	720.781984	12.671578
13.775648	724.435516	12.676595
14.033956	712.394164	12.681613
13.782555	721.682455	12.686631
13.918554	719.087327	12.691648
13.945845	710.426457	12.696666
13.898308	717.330244	12.701683
13.930285	712.721649	12.706701
13.936297	724.833878	12.711719
14.149254	726.705755	12.716736
13.901743	726.913543	12.721754
14.129788	737.786405	12.726771
14.411780	732.235721	12.731789
14.146148	721.348104	12.736807
13.897190	717.376907	12.741824
13.901519	719.930263	12.746842
13.844368	728.337907	12.751859
13.994191	736.339724	12.756877
14.140430	746.584896	12.761895
14.112116	742.524267	12.766912
14.276038	739.995749	12.771930
14.576564	763.076785	12.776947
14.280798	739.222036	12.781965
13.992440	716.569747	12.786983
14.209427	727.946962	12.792000
14.159018	720.722718	12.797018
14.114119	737.649177	12.802035
14.302468	737.617012	12.807053
14.287552	743.841815	12.812071
14.236902	751.320701	12.817088
14.710035	748.645912	12.822106
14.204117	743.073833	12.827123
14.194323	720.191392	12.832141
14.141115	727.403978	12.837159
14.339949	736.018273	12.842176
14.589554	740.350815	12.847194
14.262941	740.294802	12.852211
14.586389	737.566554	12.857229
14.302301	738.074102	12.862247
14.476245	736.611166	12.867264
14.433081	729.559914	12.872282
14.019346	734.382209	12.877299
14.501339	741.540488	12.882317
14.394774	738.793365	12.887335
14.167032	742.183272	12.892352
14.566386	737.232131	12.897370
14.294180	743.633547	12.902387
14.422098	740.219541	12.907405
14.457892	739.386020	12.912423
14.573272	744.772886	12.917440
14.472443	745.442087	12.922458
14.335366	749.098206	12.927475
14.271014	741.972719	12.932493
14.505278	747.245935	12.937511
14.231339	744.483523	12.942528
14.420060	754.722624	12.947546
14.245034	748.332212	12.952563
14.540781	766.227600	12.957581
14.697905	781.966474	12.962599
14.660012	780.948559	12.967616
14.691826	766.710121	12.972634
14.551901	783.920909	12.977651
14.639291	767.996970	12.982669
14.671997	766.744108	12.987687
14.621002	779.523880	12.992704
14.616934	766.445659	12.997722
14.611298	770.079345	13.002739
14.866209	767.965394	13.007757
15.039381	767.991064	13.012775
14.828696	773.892340	13.017792
15.067100	769.072067	13.022810
15.233237	779.119873	13.027827
15.077815	769.789386	13.032845
15.135083	764.455952	13.037863
14.930028	755.454961	13.042880
14.985572	745.088510	13.047898
14.949989	735.472200	13.052915
14.729266	738.102529	13.057933
14.737298	746.834168	13.062951
14.719545	760.543767	13.067968
15.018637	764.133495	13.072986
15.092289	772.846762	13.078003
15.327080	776.686928	13.083021
14.965989	749.215908	13.088039
14.491863	761.425882	13.093056
14.819088	752.974173	13.098074
14.767151	768.137391	13.103091
14.839055	767.393333	13.108109
15.062784	766.326619	13.113127
14.749343	767.976370	13.118144
15.046499	763.985252	13.123162
15.011514	772.261291	13.128179
15.047469	769.272576	13.133197
15.158215	771.805694	13.138215
14.725462	771.031349	13.143232
14.789183	759.426017	13.148250
14.765249	770.075054	13.153267
14.963333	780.782465	13.158285
15.363438	797.000224	13.163303
15.228392	800.446189	13.168320
15.392195	793.002067	13.173338
15.447216	792.349784	13.178355
15.596069	789.397020	13.183373
15.368975	803.272742	13.188391
15.303125	794.909768	13.193408
15.271352	776.653027	13.198426
15.159590	776.682359	13.203443
15.516950	782.154009	13.208461
15.527474	778.189467	13.213479
15.447751	773.641936	13.218496
15.055596	770.934007	13.223514
15.502246	792.138564	13.228531
15.386236	778.850214	13.233549
15.688532	786.825730	13.238567
15.255212	778.306337	13.243584
15.468425	779.792574	13.248602
15.330347	784.647015	13.253619
15.505940	789.289489	13.258637
15.438836	791.109701	13.263655
15.444718	793.222880	13.268672
15.525970	780.864471	13.273690
15.524163	798.131447	13.278707
15.740833	800.753650	13.283725
15.629632	794.196913	13.288743
15.635069	798.894638	13.293760
15.812982	787.914749	13.298778
15.789764	787.283738	13.303795
15.702340	776.562118	13.308813
15.354190	767.077262	13.313831
15.752601	779.170766	13.318848
15.678890	770.294186	13.323866
15.730129	778.557078	13.328883
15.486407	792.456616	13.333901
15.638476	783.356490	13.338919
15.548888	789.612816	13.343936
15.696192	788.051948	13.348954
15.882066	793.366882	13.353971
16.104283	790.133044	13.358989
15.901762	784.617995	13.364007
15.803278	796.389602	13.369024
15.971712	791.806133	13.374042
15.849733	792.339491	13.379059
15.628097	793.485042	13.384077
15.583115	790.143264	13.389095
15.815420	796.795666	13.394112
16.265030	791.216708	13.399130
15.896004	779.906501	13.404147
15.747254	790.415678	13.409165
15.927014	781.415668	13.414183
15.700969	800.392638	13.419200
16.316111	791.568075	13.424218
15.960762	796.492882	13.429235
15.995101	796.271370	13.434253
15.888949	789.074074	13.439271
15.835502	790.594005	13.444288
15.753899	782.203146	13.449306
16.233601	794.752213	13.454323
15.951355	794.057963	13.459341
15.996613	784.302013	13.464359
15.920632	800.209956	13.469376
15.862835	792.071220	13.474394
16.112385	787.251845	13.479411
15.672820	790.740548	13.484429
15.956405	782.781083	13.489447
15.948927	797.489333	13.494464
16.137429	799.141086	13.499482
16.536390	802.121547	13.504499
16.110455	804.392321	13.509517
16.154903	796.818833	13.514535
16.381696	804.495118	13.519552
16.321313	801.230695	13.524570
16.237969	795.477934	13.529587
16.077674	795.122248	13.534605
16.592872	801.683148	13.539623
16.397596	800.802209	13.544640
16.193902	806.622223	13.549658
16.394560	799.414279	13.554675
16.562132	815.891362	13.559693
16.255945	802.086015	13.564711
15.873493	797.737603	13.569728
16.212315	809.315676	13.574746
16.543204	817.939169	13.579763
16.402634	819.877100	13.584781
16.930881	819.093015	13.589799
16.734373	819.758832	13.594816
16.434271	807.247266	13.599834
16.788213	816.308826	13.604851
16.507054	812.373663	13.609869
16.729251	796.745376	13.614887
16.507497	806.351799	13.619904
16.475289	792.576705	13.624922
16.515792	805.956801	13.629939
16.411503	816.645799	13.634957
16.863064	809.704592	13.639975
16.672571	816.232210	13.644992
16.611214	815.399677	13.650010
16.957147	817.479172	13.655027
16.566593	805.331241	13.660045
16.799203	803.238904	13.665063
16.251278	798.858156	13.670080
16.409636	807.948873	13.675098
16.721060	810.382111	13.680115
16.600011	817.151911	13.685133
16.496883	814.292006	13.690151
16.694370	811.889582	13.695168
16.673809	824.118896	13.700186
17.231419	816.124695	13.705203
16.787887	810.644576	13.710221
17.092792	810.211766	13.715239
16.536366	821.257788	13.720256
16.586495	821.963708	13.725274
16.733257	810.072703	13.730291
16.548038	816.575234	13.735309
16.774944	812.293044	13.740327
16.927763	813.208652	13.745344
16.646006	825.153844	13.750362
17.102562	827.533831	13.755379
17.046538	839.965693	13.760397
17.093718	828.573674	13.765415
17.259519	842.637851	13.770432
17.174544	827.885339	13.775450
17.242742	815.552102	13.780467
17.128985	811.272797	13.785485
17.136567	803.800899	13.790503
17.002095	805.101243	13.795520
16.929140	811.644164	13.800538
17.116966	807.949338	13.805555
17.111184	810.211692	13.810573
17.407132	822.075623	13.815591
17.055005	815.744145	13.820608
16.864177	805.891997	13.825626
17.458517	821.263183	13.830643
17.433083	833.866322	13.835661
17.162903	821.897176	13.840679
17.513704	807.044695	13.845696
16.980863	819.950649	13.850714
17.376929	807.883178	13.855731
17.475733	815.450041	13.860749
17.283910	823.035491	13.865767
17.272587	810.433998	13.870784
17.364675	825.626874	13.875802
17.457795	824.280113	13.880819
17.371782	827.669118	13.885837
17.455210	820.934557	13.890855
17.469290	822.734193	13.895872
17.239429	829.646092	13.900890
17.620594	823.591129	13.905907
17.676441	845.582912	13.910925
17.557195	823.493657	13.915943
17.281746	820.144512	13.920960
17.046361	833.834447	13.925978
17.185990	836.575754	13.930995
17.488036	832.191311	13.936013
17.426757	830.601332	13.941031
17.558344	824.818151	13.946048
17.523476	828.456119	13.951066
17.288978	829.968354	13.956083
17.080822	840.954732	13.961101
17.043123	834.862698	13.966119
17.242073	851.909764	13.971136
17.272888	862.125382	13.976154
18.055041	858.977586	13.981171
18.386326	859.997384	13.986189
18.535229	848.369953	13.991207
18.050726	832.637058	13.996224
17.873567	827.244541	14.001242
17.829008	826.765884	14.006259
18.060483	824.484376	14.011277
18.118377	824.259145	14.016295
17.697148	818.437937	14.021312
17.767111	828.601360	14.026330
18.093146	825.786846	14.031347
17.537423	823.974739	14.036365
17.545482	821.195754	14.041383
17.954085	814.350065	14.046400
17.791341	836.500994	14.051418
18.164639	825.160672	14.056435
17.606327	833.961297	14.061453
17.653376	835.511770	14.066471
17.393591	844.432457	14.071488
17.855315	842.807907	14.076506
18.053087	839.337980	14.081523
17.826336	854.282323	14.086541
17.708332	850.702291	14.091559
18.037556	840.824309	14.096576
17.999111	858.803302	14.101594
18.338586	851.874211	14.106611
18.306190	841.252054	14.111629
18.163448	849.345468	14.116647
18.134535	843.003561	14.121664
18.140740	858.328452	14.126682
18.435503	846.183110	14.131699
18.460124	849.215170	14.136717
18.352763	850.220086	14.141735
18.466712	851.088223	14.146752
18.230939	858.035367	14.151770
18.597746	838.689142	14.156787
18.574421	851.600586	14.161805
18.668212	845.415438	14.166823
18.489249	843.073414	14.171840
18.329489	849.869346	14.176858
18.556748	841.869610	14.181875
18.622811	840.417903	14.186893
18.606133	841.347120	14.191911
18.848429	838.921300	14.196928
18.459668	845.714744	14.201946
18.481798	840.733165	14.206963
18.654492	844.037444	14.211981
17.990373	830.901957	14.216999
18.189122	838.060316	14.222016
18.503161	845.456586	14.227034
19.132383	834.429603	14.232051
19.004077	849.006420	14.237069
18.770816	832.393630	14.242087
18.450347	815.369397	14.247104
18.236606	827.486541	14.252122
18.484499	844.936855	14.257139
18.407484	845.841063	14.262157
18.476427	848.630339	14.267175
18.811305	837.834548	14.272192
18.584742	846.120621	14.277210
18.537057	842.413163	14.282227
18.696442	847.721889	14.287245
18.729959	853.525523	14.292263
18.697841	848.853332	14.297280
18.566085	843.488300	14.302298
18.708629	840.857814	14.307315
18.650780	847.772625	14.312333
18.552035	848.147802	14.317351
19.032495	847.452362	14.322368
18.904111	864.377088	14.327386
19.142464	865.696173	14.332403
19.012653	849.735026	14.337421
18.579871	848.990208	14.342439
19.085166	861.006763	14.347456
18.874274	865.939272	14.352474
18.972406	877.074361	14.357491
18.976081	869.467656	14.362509
19.067931	880.243185	14.367527
19.362680	857.924451	14.372544
19.323103	867.104201	14.377562
18.895280	873.181753	14.382579
19.254178	869.643703	14.387597
19.325116	871.640575	14.392615
19.524060	855.245276	14.397632
19.043442	841.906456	14.402650
19.221150	836.022304	14.407667
19.260868	830.519333	14.412685
19.066746	843.814649	14.417703
19.221409	838.118566	14.422720
19.220273	849.590587	14.427738
19.265176	855.665934	14.432755
19.212622	849.140171	14.437773
19.196879	862.353495	14.442791
19.396400	860.696151	14.447808
19.690736	859.396253	14.452826
19.677804	862.295984	14.457843
19.362804	839.531807	14.462861
19.429909	834.909265	14.467879
19.434519	821.107555	14.472896
19.233404	831.935286	14.477914
19.145944	839.108542	14.482931
19.389348	851.571743	14.487949
19.166565	859.545797	14.492967
19.306074	864.064182	14.497984
19.166539	865.385450	14.503002
19.427454	860.876741	14.508019
19.483440	866.729005	14.513037
19.185241	865.983075	14.518055
19.681416	859.004315	14.523072
19.566556	857.031532	14.528090
19.414405	857.075843	14.533107
19.490636	859.974532	14.538125
19.597549	865.132153	14.543143
19.784362	876.677280	14.548160
19.744127	890.039177	14.553178
19.895832	887.868550	14.558195
19.855384	864.593377	14.563213
19.825899	858.161801	14.568231
19.891226	866.430076	14.573248
19.868470	855.539000	14.578266
19.806419	870.092621	14.583283
19.873301	853.063803	14.588301
19.744485	862.996525	14.593319
19.773963	855.803228	14.598336
19.780561	864.159605	14.603354
19.806937	890.023037	14.608371
19.982321	885.111634	14.613389
20.004502	895.666484	14.618407
20.185507	889.566816	14.623424
20.334840	891.945912	14.628442
19.828040	882.906028	14.633459
20.161780	867.785476	14.638477
19.970407	888.068126	14.643495
20.220084	877.646289	14.648512
20.364107	876.283584	14.653530
19.922717	872.644311	14.658547
20.242290	862.420697	14.663565
19.842754	876.296998	14.668583
20.250477	874.297193	14.673600
20.160750	891.594634	14.678618
20.247830	898.446798	14.683635
20.128053	885.442429	14.688653
20.020989	899.378006	14.693671
19.997668	886.793405	14.698688
20.100717	886.973241	14.703706
19.703892	893.555461	14.708723
20.153995	897.121105	14.713741
20.336590	892.436441	14.718759
20.252665	891.703711	14.723776
20.191127	885.406577	14.728794
19.766660	895.955354	14.733811
20.321969	896.878869	14.738829
20.467351	917.989390	14.743847
20.428895	910.494780	14.748864
20.788641	911.093341	14.753882
20.781312	912.194619	14.758899
20.879941	900.273949	14.763917
20.555814	900.256692	14.768935
20.545162	889.186426	14.773952
20.409897	891.046718	14.778970
20.420901	908.657730	14.783987
20.902932	903.998091	14.789005
21.147945	900.963580	14.794023
20.965230	889.646732	14.799040
20.931194	878.320534	14.804058
20.747214	885.807473	14.809075
20.817746	872.806914	14.814093
20.371215	875.999962	14.819111
20.722004	874.876102	14.824128
20.637172	878.066115	14.829146
20.510812	878.540759	14.834163
20.711722	871.914199	14.839181
20.773361	891.504841	14.844199
20.998546	900.990190	14.849216
21.202404	908.059156	14.854234
20.682906	892.447363	14.859251
20.903287	884.995565	14.864269
20.870554	903.877149	14.869287
20.853290	907.923209	14.874304
21.112484	901.246401	14.879322
20.905985	903.661808	14.884339
21.251107	901.566505	14.889357
20.961951	894.443079	14.894375
21.003172	906.099428	14.899392
21.249248	899.863358	14.904410
20.756263	899.518283	14.909427
21.172201	898.457998	14.914445
20.804002	897.030829	14.919463
20.893179	892.740409	14.924480
21.066986	885.121559	14.929498
20.858370	903.170224	14.934515
21.213752	900.824806	14.939533
20.962774	906.588350	14.944551
21.011573	905.169426	14.949568
21.205862	895.513038	14.954586
20.760266	908.120328	14.959603
21.127594	918.261943	14.964621
21.249965	928.995033	14.969639
21.688530	929.657262	14.974656
21.926731	920.696667	14.979674
21.406951	914.430806	14.984691
21.576706	897.977325	14.989709
21.467847	890.732994	14.994727
21.483315	897.758074	14.999744
21.596822	901.530444	15.004762
21.266610	902.764911	15.009779
21.627321	895.213804	15.014797
21.468930	899.611645	15.019815
21.373023	899.508427	15.024832
21.915405	903.139439	15.029850
21.435147	908.680085	15.034867
21.676839	902.076260	15.039885
21.884019	917.496539	15.044903
21.798514	915.968842	15.049920
21.826029	909.201412	15.054938
21.615311	905.900540	15.059955
21.796770	898.477251	15.064973
21.599744	893.547827	15.069991
21.487011	903.644033	15.075008
21.677672	909.362912	15.080026
21.407382	929.729595	15.085043
21.590830	927.577701	15.090061
21.675457	930.181718	15.095079
21.742581	939.232759	15.100096
22.144319	930.376860	15.105114
21.984763	932.717543	15.110131
21.841920	930.445876	15.115149
21.542632	926.563299	15.120167
21.886365	935.496713	15.125184
22.003435	929.729291	15.130202
22.030973	936.628375	15.135219
22.171303	932.896337	15.140237
22.218544	919.501209	15.145255
21.837358	927.231956	15.150272
22.390284	927.634246	15.155290
22.271218	929.482795	15.160307
22.215481	924.910170	15.165325
22.185306	922.073747	15.170343
21.853509	930.168312	15.175360
22.060514	920.044467	15.180378
22.137904	922.780387	15.185395
22.229942	920.529127	15.190413
22.303497	934.174100	15.195431
22.059133	928.960424	15.200448
22.470519	915.683111	15.205466
22.361019	926.934238	15.210483
22.327081	917.690944	15.215501
22.350727	915.829376	15.220519
22.185894	930.307228	15.225536
22.515125	929.352292	15.230554
22.232147	935.486498	15.235571
22.302498	953.030219	15.240589
22.435208	950.012790	15.245607
22.441078	964.250896	15.250624
22.468185	946.949861	15.255642
22.517037	956.285035	15.260659
22.909533	946.778732	15.265677
23.085862	942.989924	15.270695
22.722208	941.360039	15.275712
22.580038	920.542492	15.280730
22.649181	925.260375	15.285747
22.725941	917.163968	15.290765
22.739639	924.322024	15.295783
22.538482	929.790698	15.300800
22.995323	936.540873	15.305818
22.787599	935.711008	15.310835
22.802710	926.071784	15.315853
22.775675	931.220984	15.320871
22.585245	933.820328	15.325888
23.023832	940.507007	15.330906
22.781072	942.100936	15.335923
22.794276	947.138734	15.340941
23.133825	943.936148	15.345959
22.844702	947.272329	15.350976
23.167494	943.968597	15.355994
23.205380	943.472691	15.361011
23.081723	939.530606	15.366029
23.111186	935.547326	15.371047
23.327871	936.886554	15.376064
23.311953	920.412731	15.381082
22.671572	913.340586	15.386099
22.642539	926.297921	15.391117
23.388692	933.760594	15.396135
23.197164	942.482995	15.401152
23.147147	935.935121	15.406170
23.254078	939.158624	15.411187
23.166669	945.931944	15.416205
23.440664	922.569382	15.421223
23.384891	946.727767	15.426240
23.508279	939.353872	15.431258
23.573893	938.904929	15.436275
23.033079	935.186502	15.441293
23.361739	926.816346	15.446311
23.400617	936.288197	15.451328
23.598176	929.327544	15.456346
23.493106	937.368682	15.461363
23.400919	937.363265	15.466381
23.500385	931.504286	15.471399
23.564122	941.546384	15.476416
23.518860	935.440608	15.481434
23.793648	930.312680	15.486451
23.348383	931.258416	15.491469
23.724603	925.386115	15.496487
23.380213	935.669262	15.501504
23.444296	946.142777	15.506522
23.636019	939.739750	15.511539
23.567790	951.864694	15.516557
23.658679	934.785735	15.521575
23.455284	927.076813	15.526592
23.469317	933.408882	15.531610
23.607158	930.583111	15.536627
23.342307	938.243350	15.541645
23.419955	938.997848	15.546663
23.232789	936.968966	15.551680
23.768128	957.969456	15.556698
23.661741	958.767535	15.561715
23.607302	970.389442	15.566733
24.030862	959.702049	15.571751
24.057974	966.610665	15.576768
24.131472	958.995066	15.581786
24.449553	971.116837	15.586803
24.310139	959.185295	15.591821
24.540400	958.118861	15.596839
24.181443	943.315325	15.601856
24.125619	939.830049	15.606874
24.025446	932.804320	15.611891
23.947460	927.849982	15.616909
23.981727	932.200063	15.621927
23.925337	939.768571	15.626944
23.814917	958.465115	15.631962
24.283385	960.030591	15.636979
24.141733	968.695114	15.641997
24.216645	969.134732	15.647015
24.253864	962.002300	15.652032
24.316489	964.808001	15.657050
24.394640	959.064358	15.662067
24.252238	963.767810	15.667085
24.594847	974.732422	15.672103
24.189606	963.781227	15.677120
24.410713	974.034185	15.682138
24.753493	972.313257	15.687155
24.444632	960.625220	15.692173
24.617298	968.122996	15.697191
24.319801	967.255690	15.702208
24.358388	969.522110	15.707226
24.648579	971.009745	15.712243
24.136502	969.309256	15.717261
24.473357	966.049636	15.722279
24.177838	960.592890	15.727296
24.606035	969.327257	15.732314
24.819620	983.650142	15.737331
24.505590	984.572887	15.742349
25.004700	985.913994	15.747367
24.835560	984.291930	15.752384
24.866046	987.361229	15.757402
25.044090	981.613967	15.762419
24.691469	970.909125	15.767437
24.826471	962.508542	15.772455
24.747717	973.691211	15.777472
25.141457	991.622147	15.782490
25.067595	979.142322	15.787507
24.876214	977.761737	15.792525
24.888910	990.898401	15.797543
24.907204	977.073805	15.802560
25.024038	988.554273	15.807578
25.131569	979.079959	15.812595
24.761903	987.191478	15.817613
25.064618	982.767514	15.822631
25.285504	992.083958	15.827648
25.070235	994.715786	15.832666
25.137446	982.288884	15.837683
25.222579	987.634015	15.842701
25.271148	977.005787	15.847719
25.227468	982.203437	15.852736
25.150995	987.381738	15.857754
25.206131	982.416673	15.862771
25.124435	987.542301	15.867789
24.967251	986.603645	15.872807
24.870330	988.032401	15.877824
24.973372	976.438479	15.882842
25.287321	983.671848	15.887859
25.305824	1004.897667	15.892877
25.610888	1009.980673	15.897895
25.638460	1013.961044	15.902912
25.595142	1003.953550	15.907930
25.587119	976.791924	15.912947
25.091804	1001.307292	15.917965
25.709197	996.769215	15.922983
25.446744	999.517541	15.928000
25.773253	1007.477535	15.933018
25.862748	1006.212853	15.938035
25.973485	1014.824429	15.943053
25.645791	1001.079364	15.948071
25.771405	994.796352	15.953088
25.687278	1012.525651	15.958106
25.720675	1013.096967	15.963123
25.312517	1009.111211	15.968141
25.492493	1011.906470	15.973159
25.639173	1011.940481	15.978176
26.015228	1010.467942	15.983194
26.170137	999.947214	15.988211
26.066580	1005.693772	15.993229
25.913664	997.012696	15.998247
26.153068	1005.037163	16.003264
25.711054	993.080697	16.008282
26.020215	1009.163214	16.013299
25.371135	1005.697791	16.018317
25.475005	1013.561729	16.023335
26.000608	1011.726951	16.028352
26.216735	1020.609187	16.033370
26.606502	1034.049338	16.038387
26.591096	1016.799383	16.043405
26.153211	1006.231516	16.048423
26.409446	999.589409	16.053440
26.144175	1004.375496	16.058458
25.905342	993.320247	16.063475
26.136887	1003.376225	16.068493
26.496005	1013.548006	16.073511
26.612141	1005.693814	16.078528
26.125318	1016.702619	16.083546
26.713629	1017.997015	16.088563
26.470434	1017.692699	16.093581
26.092599	1023.199825	16.098599
26.412832	1010.401337	16.103616
26.486633	1029.411423	16.108634
26.458167	1018.566455	16.113651
26.831385	1022.032316	16.118669
26.924793	1016.753415	16.123687
26.875504	1029.173680	16.128704
26.492371	1007.021729	16.133722
26.834254	1011.445108	16.138739
26.397643	1018.383186	16.143757
26.762556	1006.711073	16.148775
26.974540	1016.454185	16.153792
26.658227	1014.775874	16.158810
27.106002	1022.852722	16.163827
26.863044	1007.531444	16.168845
26.708473	999.125824	16.173863
27.175339	1005.040944	16.178880
26.849943	1000.556421	16.183898
26.683647	988.567122	16.188915
27.145664	997.368321	16.193933
26.739940	998.292528	16.198951
26.870518	1016.670361	16.203968
26.928923	1023.004147	16.208986
26.903898	1024.789047	16.214003
27.259567	1015.654158	16.219021
26.959594	1022.673066	16.224039
27.182221	1013.422896	16.229056
26.969591	1023.523580	16.234074
27.417843	1022.913011	16.239091
27.233638	1020.214763	16.244109
27.008141	1023.681715	16.249127
27.333538	1009.752507	16.254144
27.082997	1016.115199	16.259162
26.908191	1007.461376	16.264179
27.002993	1020.780865	16.269197
26.837629	1024.584262	16.274215
27.050757	1024.947762	16.279232
27.390437	1048.323687	16.284250
27.131354	1046.600035	16.289267
26.978702	1038.791288	16.294285
27.343018	1051.603434	16.299303
27.429075	1052.364808	16.304320
27.482858	1050.087999	16.309338
27.635112	1040.085375	16.314355
27.633508	1048.762097	16.319373
27.403423	1053.764386	16.324391
27.818241	1040.724179	16.329408
27.663313	1051.019611	16.334426
27.800695	1044.113394	16.339443
27.614633	1035.307104	16.344461
27.612955	1043.139390	16.349479
27.775691	1034.143244	16.354496
27.431630	1051.245353	16.359514
27.891420	1040.482201	16.364531
27.843146	1047.541171	16.369549
27.135378	1045.362594	16.374567
27.928417	1051.597517	16.379584
28.339108	1053.095445	16.384602
28.582097	1064.616022	16.389619
28.398217	1045.809864	16.394637
28.241549	1037.392367	16.399655
28.341154	1029.734601	16.404672
28.161693	1032.274267	16.409690
28.243125	1033.351747	16.414707
28.486167	1025.992173	16.419725
28.424263	1024.069225	16.424743
28.353590	1028.103721	16.429760
28.468595	1033.118723	16.434778
28.300938	1023.507059	16.439795
28.236032	1024.539573	16.444813
28.146529	1021.099638	16.449831
28.431831	1019.808710	16.454848
28.469425	1042.380155	16.459866
28.335073	1032.333052	16.464883
28.531634	1026.255940	16.469901
28.304571	1029.862911	16.474919
28.253002	1019.609940	16.479936
28.262750	1032.753429	16.484954
28.519805	1029.971996	16.489971
28.289048	1024.200936	16.494989
28.178260	1033.254438	16.500007
28.384246	1041.891929	16.505024
28.534538	1058.761494	16.510042
28.659335	1054.675728	16.515059
28.718660	1050.693754	16.520077
28.682868	1053.816206	16.525095
29.148620	1047.726627	16.530112
28.783897	1049.929390	16.535130
28.635982	1055.332962	16.540147
28.670225	1049.525328	16.545165
28.710661	1051.540678	16.550183
28.617163	1045.868444	16.555200
28.645469	1043.001806	16.560218
28.841839	1052.827848	16.565235
29.122765	1042.237330	16.570253
28.984028	1054.764605	16.575271
29.045178	1044.513354	16.580288
28.917888	1051.485071	16.585306
29.249504	1056.495966	16.590323
29.203609	1051.028799	16.595341
28.949635	1045.064356	16.600359
29.265302	1050.662123	16.605376
28.987408	1059.272178	16.610394
28.751499	1039.957377	16.615411
28.988197	1048.265374	16.620429
28.857585	1054.536892	16.625447
28.653396	1059.490788	16.630464
28.967380	1072.416429	16.635482
29.177209	1082.562678	16.640499
29.430829	1083.075348	16.645517
29.203490	1084.549410	16.650535
29.803671	1075.204957	16.655552
29.664414	1077.366706	16.660570
29.644480	1081.632929	16.665587
29.802064	1078.533785	16.670605
29.676896	1067.952874	16.675623
29.800407	1075.693900	16.680640
29.794272	1079.126768	16.685658
29.619318	1077.065523	16.690675
29.819199	1070.421335	16.695693
29.695183	1083.904013	16.700711
29.763772	1075.445513	16.705728
29.987319	1077.233592	16.710746
29.835699	1075.503886	16.715763
29.955289	1069.748984	16.720781
29.682959	1081.399316	16.725799
29.874990	1068.805543	16.730816
29.751873	1073.596763	16.735834
29.556817	1080.643532	16.740851
29.859135	1072.056427	16.745869
30.049792	1079.069401	16.750887
30.083650	1066.834580	16.755904
29.905969	1064.761980	16.760922
29.899420	1083.799267	16.765939
30.056659	1074.850466	16.770957
29.934640	1078.614390	16.775975
29.887581	1077.460190	16.780992
30.250074	1078.387420	16.786010
30.204387	1078.019961	16.791027
29.967405	1069.250459	16.796045
30.165800	1076.329071	16.801063
30.461463	1083.561985	16.806080
30.448457	1094.219664	16.811098
30.556545	1096.014731	16.816115
30.653742	1087.227469	16.821133
30.282223	1077.735084	16.826151
30.721680	1082.815461	16.831168
30.677709	1072.839526	16.836186
30.301638	1073.748966	16.841203
30.473794	1058.130307	16.846221
30.396292	1076.016444	16.851239
30.583814	1083.957062	16.856256
31.108353	1095.228908	16.861274
30.728790	1088.364893	16.866291
30.695115	1069.159743	16.871309
30.885087	1068.608635	16.876327
30.626553	1068.913923	16.881344
30.761932	1064.408699	16.886362
30.876109	1072.591804	16.891379
30.598164	1058.016412	16.896397
30.634976	1080.499072	16.901415
30.819456	1084.126232	16.906432
30.878442	1093.086594	16.911450
31.013129	1110.023767	16.916467
31.191637	1094.980367	16.921485
31.346441	1084.943041	16.926503
31.024355	1087.219033	16.931520
31.109709	1071.841549	16.936538
31.232465	1086.463864	16.941555
31.343611	1089.043030	16.946573
30.849707	1078.257662	16.951591
30.997703	1081.403115	16.956608
31.332544	1086.951253	16.961626
30.928559	1086.499258	16.966643
31.257820	1087.436343	16.971661
31.020038	1095.171290	16.976679
31.026092	1093.519701	16.981696
31.138707	1092.280302	16.986714
31.141245	1098.185629	16.991731
31.073670	1094.338509	16.996749
31.208489	1105.978273	17.001767
31.376507	1110.970316	17.006784
31.818253	1120.553265	17.011802
31.657070	1127.256252	17.016819
31.791485	1121.983097	17.021837
31.681529	1121.170828	17.026855
31.607903	1118.525440	17.031872
31.791167	1120.174950	17.036890
31.644805	1122.902034	17.041907
31.969719	1116.408297	17.046925
31.673575	1115.384072	17.051943
31.848223	1122.758371	17.056960
32.018180	1118.121013	17.061978
31.478855	1125.807672	17.066995
31.766331	1114.540063	17.072013
31.609993	1113.903213	17.077031
31.658052	1118.388449	17.082048
32.156923	1115.982539	17.087066
32.026382	1120.867129	17.092083
32.079900	1118.993879	17.097101
32.213079	1116.550722	17.102119
31.967811	1116.507365	17.107136
32.418051	1110.036893	17.112154
31.741392	1115.501203	17.117171
31.971393	1114.524169	17.122189
32.319215	1113.152372	17.127207
31.927056	1119.313851	17.132224
32.008769	1107.540708	17.137242
32.351969	1128.785955	17.142259
32.333191	1128.114430	17.147277
32.372079	1134.707399	17.152295
32.501072	1140.836596	17.157312
32.491398	1136.568049	17.162330
32.484212	1135.858378	17.167347
32.621675	1129.791443	17.172365
32.616540	1134.259542	17.177383
32.436564	1134.066363	17.182400
32.558382	1125.576549	17.187418
32.307165	1138.687521	17.192435
32.449094	1136.370066	17.197453
32.907886	1133.830663	17.202471
32.443314	1134.040675	17.207488
32.657284	1125.809942	17.212506
32.382081	1129.697365	17.217523
32.580555	1132.199821	17.222541
32.545843	1130.179430	17.227559
32.697119	1143.970326	17.232576
32.962682	1150.613025	17.237594
32.704974	1169.098093	17.242611
32.774270	1163.075150	17.247629
33.028433	1166.596658	17.252647
32.839906	1161.833444	17.257664
33.405026	1152.735313	17.262682
33.393576	1154.025868	17.267699
33.326021	1152.058963	17.272717
33.450247	1150.435363	17.277735
33.084806	1167.412812	17.282752
33.623700	1154.717226	17.287770
33.201016	1157.415835	17.292787
33.254764	1156.469274	17.297805
33.451579	1154.158048	17.302823
33.417557	1160.650946	17.307840
33.391252	1153.222699	17.312858
33.099210	1153.307189	17.317875
33.361134	1152.080369	17.322893
33.318585	1150.781719	17.327911
33.517610	1161.691594	17.332928
33.587603	1149.514478	17.337946
32.919190	1167.331224	17.342963
32.841853	1164.573458	17.347981
33.271769	1176.153991	17.352999
33.308265	1180.953753	17.358016
33.394999	1188.022630	17.363034
33.758058	1187.147881	17.368051
33.772989	1182.561072	17.373069
33.741657	1177.331193	17.378087
33.774521	1188.271853	17.383104
33.807310	1170.966868	17.388122
33.861566	1184.864079	17.393139
33.994320	1201.548928	17.398157
34.370246	1199.980335	17.403175
34.271200	1197.611195	17.408192
34.347760	1170.705238	17.413210
34.255964	1175.833788	17.418227
34.149162	1174.700139	17.423245
34.261580	1172.169483	17.428263
34.183744	1176.219775	17.433280
34.330710	1176.469085	17.438298
34.132110	1172.308304	17.443315
34.156812	1173.629464	17.448333
34.303101	1162.796687	17.453351
34.042215	1171.435866	17.458368
34.327432	1184.627789	17.463386
34.306077	1200.606392	17.468403
34.433064	1204.678552	17.473421
35.054130	1193.351899	17.478439
34.813128	1197.990316	17.483456
35.024323	1192.694927	17.488474
34.797020	1182.313583	17.493491
34.590213	1176.247158	17.498509
35.112075	1159.731334	17.503527
34.408960	1163.520603	17.508544
34.959600	1158.845157	17.513562
35.226270	1162.858658	17.518579
34.901418	1155.932372	17.523597
34.995715	1155.684945	17.528615
34.655145	1156.960520	17.533632
34.618247	1165.581365	17.538650
34.673245	1162.741370	17.543667
34.531069	1167.089349	17.548685
34.867548	1166.661125	17.553703
34.669174	1186.373701	17.558720
35.353642	1191.785031	17.563738
35.271703	1204.281727	17.568755
35.073869	1204.057264	17.573773
35.380900	1197.902672	17.578791
35.119273	1198.103362	17.583808
34.990481	1184.402236	17.588826
35.055695	1190.938887	17.593843
34.884294	1188.902233	17.598861
35.218634	1185.024508	17.603879
35.078313	1187.199048	17.608896
35.144769	1190.578932	17.613914
35.634489	1189.306374	17.618931
35.298903	1185.259299	17.623949
35.499614	1180.234543	17.628967
35.163441	1203.524618	17.633984
35.698612	1210.498895	17.639002
35.917794	1220.825169	17.644019
35.845926	1220.293561	17.649037
35.855769	1211.625862	17.654055
35.432882	1200.603811	17.659072
35.355762	1214.402416	17.664090
35.709236	1212.763148	17.669107
35.360168	1219.264734	17.674125
36.159478	1208.407637	17.679143
35.606402	1218.745733	17.684160
35.653614	1215.914109	17.689178
35.800432	1219.894398	17.694195
35.381022	1223.041669	17.699213
35.984415	1231.167563	17.704231
36.112380	1243.002262	17.709248
36.486775	1246.309718	17.714266
36.270218	1240.993679	17.719283
36.351982	1243.804123	17.724301
36.800818	1218.766450	17.729319
36.564688	1215.063845	17.734336
36.266380	1219.854307	17.739354
36.602456	1199.330110	17.744371
36.165322	1214.989267	17.749389
36.187084	1208.019521	17.754407
36.329703	1213.264234	17.759424
35.996823	1208.938367	17.764442
36.324214	1226.744391	17.769459
36.586495	1239.324056	17.774477
36.745808	1242.535768	17.779495
36.787051	1242.375502	17.784512
36.843738	1253.229574	17.789530
36.879037	1239.451521	17.794547
36.687102	1243.669214	17.799565
36.934349	1239.834691	17.804583
36.627017	1240.451623	17.809600
37.049839	1244.632886	17.814618
36.908392	1231.304674	17.819635
36.707101	1239.183621	17.824653
36.937616	1225.647140	17.829671
36.679684	1233.947294	17.834688
36.986792	1232.141327	17.839706
36.934030	1231.020738	17.844723
37.049823	1229.114291	17.849741
37.186741	1233.438735	17.854759
37.131841	1242.566926	17.859776
37.137687	1230.077586	17.864794
36.966429	1227.502735	17.869811
37.101020	1235.353413	17.874829
37.043454	1231.632149	17.879847
36.622221	1235.624181	17.884864
36.650213	1245.982249	17.889882
37.319894	1259.470166	17.894899
37.667952	1260.624996	17.899917
37.422268	1264.387078	17.904935
37.536327	1261.284109	17.909952
37.268045	1266.145970	17.914970
38.070013	1253.186509	17.919987
37.761558	1267.612960	17.925005
37.670022	1254.499258	17.930023
37.498818	1252.797195	17.935040
37.575653	1264.351837	17.940058
37.580461	1268.730137	17.945075
37.550967	1272.185433	17.950093
37.726190	1261.172193	17.955111
37.894843	1249.597476	17.960128
37.535125	1252.154933	17.965146
37.739611	1258.620829	17.970163
37.881712	1286.958906	17.975181
38.130229	1285.025275	17.980199
38.148683	1284.023550	17.985216
38.076990	1289.599174	17.990234
38.279044	1281.906934	17.995251
38.303919	1292.208073	18.000269
38.472194	1278.657876	18.005287
38.551669	1274.741784	18.010304
38.022437	1265.829805	18.015322
38.219623	1264.557046	18.020339
38.696118	1276.007477	18.025357
38.294404	1269.219501	18.030375
38.169132	1267.707432	18.035392
38.724754	1279.719104	18.040410
38.832683	1285.587302	18.045427
38.684462	1293.672016	18.050445
38.641898	1279.648216	18.055463
38.767406	1260.794310	18.060480
38.579687	1266.905333	18.065498
38.595625	1262.068342	18.070515
38.971029	1285.206415	18.075533
39.030385	1281.820418	18.080551
38.876351	1255.693557	18.085568
38.571165	1258.791537	18.090586
38.381392	1262.598261	18.095603
38.588296	1274.645053	18.100621
38.910893	1284.745529	18.105639
38.697350	1282.823736	18.110656
38.857490	1275.865211	18.115674
38.905660	1285.602652	18.120691
38.840918	1281.919575	18.125709
38.746998	1284.207671	18.130727
39.241391	1296.902737	18.135744
39.119697	1293.154716	18.140762
39.690217	1295.025698	18.145779
39.484307	1295.557274	18.150797
39.548327	1289.566260	18.155815
39.829176	1290.271256	18.160832
39.214338	1279.136568	18.165850
39.547652	1275.870782	18.170867
39.245336	1278.122650	18.175885
39.494821	1284.923192	18.180903
39.649953	1290.969761	18.185920
39.571765	1301.603772	18.190938
39.805629	1300.844975	18.195955
39.344650	1292.076750	18.200973
39.626413	1300.956900	18.205991
39.665593	1292.450810	18.211008
39.568585	1296.866905	18.216026
39.527210	1304.621672	18.221043
39.609329	1291.602301	18.226061
39.694399	1299.284477	18.231079
39.823656	1291.638976	18.236096
39.622907	1299.647386	18.241114
40.148293	1305.536363	18.246131
39.890843	1335.723554	18.251149
39.908248	1326.114406	18.256167
40.229528	1322.282519	18.261184
40.037010	1320.368250	18.266202
40.222466	1314.247204	18.271219
40.499974	1316.829072	18.276237
40.671104	1320.943531	18.281255
40.626950	1313.151256	18.286272
40.638904	1321.998312	18.291290
40.839217	1312.488690	18.296307
40.644120	1307.150952	18.301325
40.435240	1284.140139	18.306343
40.902998	1288.761962	18.311360
40.392590	1286.688728	18.316378
40.425887	1276.581712	18.321395
40.590119	1280.632349	18.326413
40.454407	1303.857761	18.331431
40.751722	1302.878977	18.336448
40.617810	1304.895386	18.341466
40.881659	1306.825214	18.346483
40.933104	1307.140400	18.351501
40.606028	1317.588238	18.356519
40.951246	1312.539816	18.361536
40.653399	1313.433905	18.366554
40.863421	1313.430619	18.371571
40.937681	1308.177635	18.376589
40.746634	1317.733996	18.381607
40.984062	1304.568333	18.386624
40.710025	1321.327221	18.391642
40.967923	1330.360563	18.396659
41.015865	1338.853234	18.401677
40.960684	1339.482197	18.406695
41.235210	1335.113606	18.411712
41.177801	1341.987620	18.416730
41.400857	1337.213817	18.421747
41.211866	1331.227438	18.426765
41.210754	1354.454177	18.431783
41.801568	1358.409132	18.436800
41.773067	1379.478322	18.441818
42.091285	1361.808764	18.446835
42.053830	1351.831958	18.451853
41.978706	1342.527147	18.456871
42.007176	1324.438480	18.461888
41.933680	1335.929188	18.466906
41.902795	1329.382691	18.471923
41.989799	1321.708765	18.476941
41.776648	1334.164384	18.481959
42.023315	1327.075711	18.486976
41.970607	1338.298013	18.491994
41.567129	1321.107494	18.497011
42.169178	1332.258369	18.502029
41.881587	1351.389151	18.507047
42.298198	1364.362940	18.512064
41.824226	1378.775665	18.517082
41.912489	1364.732407	18.522099
42.268139	1355.355204	18.527117
42.143936	1362.734803	18.532135
42.566599	1359.529737	18.537152
42.401659	1364.261857	18.542170
42.444778	1363.173747	18.547187
42.101089	1361.504670	18.552205
42.236091	1366.188908	18.557223
42.434001	1356.497381	18.562240
42.636907	1366.005224	18.567258
42.552342	1367.179999	18.572275
43.006209	1370.870720	18.577293
42.645936	1381.261914	18.582311
42.937419	1358.532385	18.587328
42.815271	1355.788331	18.592346
42.606953	1357.413582	18.597363
43.098731	1364.845917	18.602381
43.111380	1379.969867	18.607399
43.236383	1367.940125	18.612416
42.815164	1366.789824	18.617434
43.044986	1369.292621	18.622451
43.318561	1363.820276	18.627469
43.103832	1367.511886	18.632487
43.583124	1364.547793	18.637504
43.037961	1356.168707	18.642522
43.234980	1365.674773	18.647539
43.214227	1367.037362	18.652557
43.233560	1374.901756	18.657575
43.439409	1370.072143	18.662592
43.268388	1368.721994	18.667610
43.574023	1376.175823	18.672627
43.331930	1360.782005	18.677645
43.497761	1376.752513	18.682663
43.450703	1370.172467	18.687680
43.333467	1374.962408	18.692698
43.247743	1371.519798	18.697715
43.524006	1383.006345	18.702733
43.732988	1392.869090	18.707751
43.783741	1393.917050	18.712768
44.215692	1400.545195	18.717786
43.979549	1397.164979	18.722803
44.307711	1403.310784	18.727821
44.365476	1391.185903	18.732839
44.264827	1380.720777	18.737856
44.186640	1370.955841	18.742874
44.065717	1359.024852	18.747891
44.213998	1361.754580	18.752909
44.346672	1376.980229	18.757927
44.336194	1374.246744	18.762944
44.425152	1380.503553	18.767962
44.371000	1377.023412	18.772979
44.332339	1377.476801	18.777997
44.358418	1393.921722	18.783015
44.654208	1379.330194	18.788032
44.802582	1388.294768	18.793050
44.528187	1390.610907	18.798067
44.672030	1387.000614	18.803085
44.493483	1384.942680	18.808103
44.717684	1384.813026	18.813120
44.799482	1382.479546	18.818138
44.608076	1389.707339	18.823155
44.686522	1382.255666	18.828173
44.611337	1385.787871	18.833191
44.557026	1381.274320	18.838208
44.634959	1390.532879	18.843226
44.719532	1392.281103	18.848243
45.021510	1402.729955	18.853261
44.835333	1409.363991	18.858279
44.813126	1418.665194	18.863296
44.876908	1414.630812	18.868314
44.889801	1410.584417	18.873331
45.627584	1413.032323	18.878349
45.187939	1413.659441	18.883367
45.052607	1414.317869	18.888384
45.585899	1411.760137	18.893402
44.952714	1418.831846	18.898419
45.562290	1422.740788	18.903437
45.590966	1443.535215	18.908455
45.883891	1435.836851	18.913472
45.850778	1422.466846	18.918490
45.566082	1416.488861	18.923507
45.408342	1412.857429	18.928525
45.619652	1437.678470	18.933543
45.575703	1436.584748	18.938560
45.581639	1439.573575	18.943578
45.622890	1441.315619	18.948595
45.949351	1434.430165	18.953613
45.819151	1443.562328	18.958631
46.083213	1435.939625	18.963648
45.925284	1429.406721	18.968666
45.879274	1438.446150	18.973683
46.274670	1442.789897	18.978701
46.250706	1445.512047	18.983719
45.715001	1451.470354	18.988736
45.894484	1438.157913	18.993754
46.075097	1470.294159	18.998771
46.612897	1462.823581	19.003789
46.617712	1451.896401	19.008807
46.945860	1439.269075	19.013824
47.395808	1437.123999	19.018842
47.350249	1424.447382	19.023859
47.253737	1410.897377	19.028877
47.450542	1416.592198	19.033895
47.490306	1408.161141	19.038912
47.206535	1392.172265	19.043930
47.115186	1383.228383	19.048947
47.260260	1370.745316	19.053965
47.278518	1374.184824	19.058983
46.681992	1371.591655	19.064000
46.977774	1363.710180	19.069018
47.018973	1373.181126	19.074035
47.015482	1363.365198	19.079053
47.005307	1366.546840	19.084071
47.287133	1365.470630	19.089088
47.204102	1363.044078	19.094106
47.153236	1369.880405	19.099123
47.358886	1379.063007	19.104141
47.586219	1382.160298	19.109159
47.440682	1393.815773	19.114176
47.384011	1390.007711	19.119194
47.274251	1390.158359	19.124211
47.323285	1395.404516	19.129229
47.620951	1413.350339	19.134247
47.476731	1415.044468	19.139264
47.949616	1412.882985	19.144282
47.209547	1413.949000	19.149299
47.359034	1412.306608	19.154317
47.143473	1413.427177	19.159335
47.344716	1421.319234	19.164352
47.993847	1421.714215	19.169370
47.582706	1426.626640	19.174387
47.546228	1420.584957	19.179405
47.679971	1427.503222	19.184423
47.528744	1439.812023	19.189440
47.441611	1442.645063	19.194458
47.900563	1462.549914	19.199475
48.118837	1460.254761	19.204493
47.764749	1458.390162	19.209511
48.026408	1471.621680	19.214528
48.374323	1488.003369	19.219546
48.220986	1491.080487	19.224563
48.615938	1487.501664	19.229581
48.719240	1488.281059	19.234599
48.529521	1488.164689	19.239616
48.884698	1488.129405	19.244634
48.799765	1486.352349	19.249651
49.039274	1484.069017	19.254669
49.102269	1478.999734	19.259687
48.710330	1488.273847	19.264704
48.516349	1479.957583	19.269722
48.612801	1482.511305	19.274739
48.574922	1481.778373	19.279757
49.067676	1483.935528	19.284775
48.666004	1478.958039	19.289792
48.610224	1482.404759	19.294810
48.545116	1486.280186	19.299827
49.271458	1512.460598	19.304845
49.369142	1508.687087	19.309863
49.194658	1509.387852	19.314880
49.477961	1507.672817	19.319898
49.512523	1507.442401	19.324915
49.486662	1496.468320	19.329933
50.035051	1508.022723	19.334951
49.681826	1508.668157	19.339968
49.506996	1500.333345	19.344986
49.536655	1509.123630	19.350003
49.645494	1504.063647	19.355021
49.707107	1507.780226	19.360039
49.519067	1512.767406	19.365056
49.982794	1501.864310	19.370074
50.181115	1510.365940	19.375091
49.618219	1514.482765	19.380109
49.619434	1503.274657	19.385127
50.072997	1509.684302	19.390144
49.846847	1505.172110	19.395162
49.845473	1508.083426	19.400179
49.925557	1515.680320	19.405197
50.256973	1525.199973	19.410215
50.005061	1534.546115	19.415232
50.567814	1527.845360	19.420250
50.514363	1529.992122	19.425267
50.086799	1532.691605	19.430285
50.203658	1527.910198	19.435303
50.124678	1535.276062	19.440320
50.528678	1523.412031	19.445338
50.414129	1522.528457	19.450355
50.648151	1523.783757	19.455373
50.811258	1526.367746	19.460391
50.857298	1546.349206	19.465408
51.149317	1535.895483	19.470426
51.163348	1530.442989	19.475443
50.782705	1524.189574	19.480461
50.753345	1524.890235	19.485479
50.844053	1541.883616	19.490496
51.121544	1534.640517	19.495514
51.161481	1546.022765	19.500531
51.235035	1547.262611	19.505549
51.545808	1545.359940	19.510567
51.584417	1544.098161	19.515584
51.701865	1550.214873	19.520602
51.593582	1543.660283	19.525619
51.463426	1546.347740	19.530637
51.304842	1524.547084	19.535655
51.495737	1537.928213	19.540672
51.697630	1533.372037	19.545690
51.426121	1542.133263	19.550707
51.732035	1547.594253	19.555725
51.528641	1547.797472	19.560743
51.718795	1551.467501	19.565760
51.416290	1556.841823	19.570778
51.652576	1550.844518	19.575795
52.104029	1561.096592	19.580813
52.032944	1546.621393	19.585831
51.490098	1547.436924	19.590848
52.045813	1556.187835	19.595866
51.869270	1566.058074	19.600883
52.209824	1573.529423	19.605901
52.265990	1566.379392	19.610919
52.309641	1584.245192	19.615936
52.314566	1575.700545	19.620954
52.300641	1574.365213	19.625971
52.389406	1574.547827	19.630989
52.366884	1569.665952	19.636007
52.396165	1574.250110	19.641024
52.290122	1570.676189	19.646042
52.495110	1576.409865	19.651059
52.363509	1571.405569	19.656077
52.625222	1574.686552	19.661095
52.626314	1583.102499	19.666112
52.510930	1584.437922	19.671130
52.582512	1601.413682	19.676147
52.374444	1606.785317	19.681165
52.729467	1597.115559	19.686183
52.565823	1595.407870	19.691200
52.816009	1612.011442	19.696218
53.285540	1615.274429	19.701235
53.342836	1621.072038	19.706253
53.386141	1616.518573	19.711271
53.531285	1617.321730	19.716288
53.616560	1612.595545	19.721306
53.584228	1614.929752	19.726323
54.026225	1617.209927	19.731341
53.939989	1601.149423	19.736359
53.602284	1585.598044	19.741376
53.714885	1583.765312	19.746394
53.728164	1578.178676	19.751411
53.664557	1582.008602	19.756429
53.636520	1587.075511	19.761447
54.057811	1603.839217	19.766464
53.836528	1604.056039	19.771482
53.896223	1618.328715	19.776499
53.731891	1614.155425	19.781517
53.952096	1610.539870	19.786535
53.820667	1611.965362	19.791552
53.958989	1607.172883	19.796570
53.952427	1606.152461	19.801587
53.811119	1620.315241	19.806605
54.205023	1627.266734	19.811623
53.890272	1635.892287	19.816640
54.161273	1645.499614	19.821658
54.520568	1633.504742	19.826675
54.304134	1637.526615	19.831693
54.818912	1634.063669	19.836711
54.435683	1636.496749	19.841728
54.620705	1648.584084	19.846746
54.692681	1644.250253	19.851763
54.865509	1657.924249	19.856781
54.746265	1664.468923	19.861799
54.972001	1670.958233	19.866816
54.909458	1666.482187	19.871834
55.428018	1658.247794	19.876851
55.066491	1663.170156	19.881869
55.309879	1662.673536	19.886887
55.069429	1657.508959	19.891904
55.565734	1661.006480	19.896922
55.745048	1657.843769	19.901939
55.806905	1658.962341	19.906957
55.371211	1636.673338	19.911975
55.714458	1630.832239	19.916992
55.400551	1633.076634	19.922010
55.852242	1635.335517	19.927027
55.600513	1630.688171	19.932045
55.369661	1625.641692	19.937063
55.622342	1649.305821	19.942080
55.424740	1649.969883	19.947098
55.772064	1649.105994	19.952115
55.876961	1652.255184	19.957133
55.687256	1654.974209	19.962151
55.399622	1656.926055	19.967168
55.712156	1650.773521	19.972186
56.344081	1661.033463	19.977203
56.076167	1665.612318	19.982221
55.815791	1670.879284	19.987239
55.923029	1682.909496	19.992256
56.253151	1691.220818	19.997274
56.615491	1682.906077	20.002291
56.327192	1681.401772	20.007309
56.515717	1682.448900	20.012327
56.335716	1690.222569	20.017344
56.237463	1692.368139	20.022362
56.544859	1686.355027	20.027379
56.475661	1687.500895	20.032397
56.912672	1702.764866	20.037415
56.712781	1702.431681	20.042432
56.648223	1710.887743	20.047450
56.881791	1708.381353	20.052467
57.198389	1719.340586	20.057485
57.133677	1714.644416	20.062503
57.102290	1707.260447	20.067520
57.075731	1709.131114	20.072538
57.300139	1695.647601	20.077555
57.440730	1698.574728	20.082573
57.539969	1695.320988	20.087591
57.592504	1693.036419	20.092608
57.108169	1704.922056	20.097626
57.499936	1692.496549	20.102643
57.393663	1694.363927	20.107661
57.408916	1696.621734	20.112679
57.294824	1702.688013	20.117696
57.174183	1718.357277	20.122714
57.603458	1721.762410	20.127731
57.478723	1729.613133	20.132749
57.512469	1727.116722	20.137767
57.712670	1738.518539	20.142784
57.907301	1741.471732	20.147802
58.196064	1745.209277	20.152819
58.308660	1756.454802	20.157837
58.129199	1761.495359	20.162855
58.496813	1756.668663	20.167872
58.342364	1757.273590	20.172890
58.652971	1746.082782	20.177907
58.976851	1737.726767	20.182925
58.798430	1745.333273	20.187943
59.077807	1727.920934	20.192960
58.764402	1718.875969	20.197978
59.112140	1700.504669	20.202995
59.093054	1705.714222	20.208013
59.091436	1706.445319	20.213031
58.912473	1704.674810	20.218048
58.830873	1701.663720	20.223066
58.702614	1698.281649	20.228083
59.106052	1703.233184	20.233101
59.170638	1707.868207	20.238119
58.810262	1705.934149	20.243136
58.801649	1716.627748	20.248154
59.081030	1717.693243	20.253171
58.834196	1734.304356	20.258189
58.971334	1733.541537	20.263207
59.432937	1729.082690	20.268224
59.144360	1741.059441	20.273242
59.586996	1736.657288	20.278259
59.515381	1737.638995	20.283277
59.289242	1737.871980	20.288295
59.682487	1741.698063	20.293312
59.266306	1766.314081	20.298330
59.904422	1766.895945	20.303347
59.688121	1769.112719	20.308365
59.523950	1775.205067	20.313383
59.671202	1769.635466	20.318400
59.827960	1779.622099	20.323418
59.968990	1772.645662	20.328435
59.930197	1788.909659	20.333453
60.023493	1784.144294	20.338471
60.073047	1787.015703	20.343488
60.233800	1790.630440	20.348506
60.067012	1783.796102	20.353523
60.205581	1784.053512	20.358541
60.193124	1792.604108	20.363559
60.391261	1792.796893	20.368576
60.144681	1819.218660	20.373594
60.739543	1810.130563	20.378611
60.644164	1814.928423	20.383629
60.831145	1820.234869	20.388647
61.214664	1804.065372	20.393664
61.454344	1819.397689	20.398682
61.340631	1810.862393	20.403699
61.648408	1820.539308	20.408717
61.472096	1809.967963	20.413735
61.389587	1811.201091	20.418752
61.125059	1808.086525	20.423770
61.341381	1807.181802	20.428787
61.450152	1813.707935	20.433805
61.385012	1813.801170	20.438823
61.284434	1802.892834	20.443840
61.059524	1809.546863	20.448858
61.039404	1807.397580	20.453875
61.136667	1812.240195	20.458893
61.444537	1826.235990	20.463911
61.436964	1825.154698	20.468928
61.289173	1840.527022	20.473946
61.662969	1840.683528	20.478963
61.946623	1839.744779	20.483981
61.945960	1837.754463	20.488999
62.548580	1838.272939	20.494016
62.373176	1842.258517	20.499034
62.343913	1832.290670	20.504051
62.394581	1832.837887	20.509069
62.398543	1822.565311	20.514087
62.477841	1835.505797	20.519104
62.891883	1846.713886	20.524122
62.835813	1839.437894	20.529139
62.683439	1828.925943	20.534157
62.456539	1823.613782	20.539175
63.076057	1833.587319	20.544192
62.795347	1826.943155	20.549210
62.783239	1832.414190	20.554227
62.977156	1834.544685	20.559245
62.758000	1844.268245	20.564263
63.270556	1851.859570	20.569280
63.561239	1851.427920	20.574298
63.029091	1852.869245	20.579315
63.097577	1852.553264	20.584333
62.919810	1856.931759	20.589351
63.523407	1831.753994	20.594368
63.319873	1846.171022	20.599386
63.581909	1852.494533	20.604403
63.516077	1845.985909	20.609421
63.321244	1851.681019	20.614439
63.565485	1847.998030	20.619456
63.433511	1857.248840	20.624474
63.275372	1842.085076	20.629491
63.415168	1863.753726	20.634509
63.860364	1874.929493	20.639527
63.968981	1869.582420	20.644544
63.786812	1881.266790	20.649562
63.562840	1877.888776	20.654579
63.821458	1873.456144	20.659597
63.662363	1885.873692	20.664615
63.937430	1892.532851	20.669632
64.144243	1900.940765	20.674650
64.449944	1891.461306	20.679667
64.502509	1905.388580	20.684685
64.291213	1898.738361	20.689703
64.543137	1885.328458	20.694720
64.893750	1899.586901	20.699738
64.773542	1904.714902	20.704755
64.993019	1889.792664	20.709773
64.665186	1899.405974	20.714791
64.982992	1897.082406	20.719808
64.848514	1900.246627	20.724826
65.012599	1903.918711	20.729843
65.203087	1905.512382	20.734861
64.940230	1924.397631	20.739879
65.185660	1922.740028	20.744896
65.089948	1931.545484	20.749914
64.851341	1927.073821	20.754931
65.104948	1920.038451	20.759949
65.160379	1932.172743	20.764967
65.170032	1941.323293	20.769984
65.338126	1955.175111	20.775002
65.553724	1958.881561	20.780019
65.901601	1949.562382	20.785037
65.985196	1954.082901	20.790055
66.152907	1945.251151	20.795072
66.049498	1950.419682	20.800090
66.080322	1957.451354	20.805107
65.939223	1951.842603	20.810125
66.261182	1953.428996	20.815143
66.278972	1948.338726	20.820160
66.228656	1954.651199	20.825178
65.926306	1962.937861	20.830195
65.971686	1967.994267	20.835213
66.289623	1977.905814	20.840231
66.475080	1968.321489	20.845248
66.563213	1974.571590	20.850266
66.769562	1976.676417	20.855283
66.839166	1971.162564	20.860301
66.619724	1975.256677	20.865319
66.713858	1972.413573	20.870336
66.854212	1974.756929	20.875354
66.393956	1980.077298	20.880371
66.899837	1989.830450	20.885389
67.322971	1997.480017	20.890407
67.185145	1998.064866	20.895424
67.601512	1999.393052	20.900442
67.160952	2002.914466	20.905459
67.739577	2006.990913	20.910477
67.778431	1998.668743	20.915495
67.949127	1994.559749	20.920512
67.734975	1992.230482	20.925530
67.704291	1993.656194	20.930547
67.777993	1985.440446	20.935565
67.661687	1997.717899	20.940583
68.130369	1993.406230	20.945600
68.038446	1986.269593	20.950618
67.962715	1991.887873	20.955635
68.266595	1988.365413	20.960653
67.965242	1989.080590	20.965671
67.848707	1984.177988	20.970688
68.134740	1991.441672	20.975706
67.962641	1997.421642	20.980723
67.873038	1989.639730	20.985741
67.834570	2019.432796	20.990759
68.011943	2018.273902	20.995776
68.190298	2014.989229	21.000794
68.478932	2025.324580	21.005811
68.555520	2020.385540	21.010829
68.541878	2040.290940	21.015847
68.575786	2038.507060	21.020864
69.452783	2044.674115	21.025882
68.810078	2039.583349	21.030899
69.454555	2032.175483	21.035917
69.551641	2038.247741	21.040935
69.260592	2030.997719	21.045952
69.531579	2041.300974	21.050970
69.817537	2033.703476	21.055987
69.675581	2024.288100	21.061005
69.719863	2033.559329	21.066023
69.744799	2033.258063	21.071040
69.757198	2028.367877	21.076058
69.449596	2035.042438	21.081075
69.672865	2029.363260	21.086093
69.243100	2038.830995	21.091111
69.662588	2034.482214	21.096128
69.848118	2032.440850	21.101146
69.772422	2037.687482	21.106163
69.795718	2030.628133	21.111181
70.067378	2051.387718	21.116199
69.858250	2054.828160	21.121216
70.339298	2047.404928	21.126234
69.962180	2056.779671	21.131251
70.308031	2047.675734	21.136269
70.007377	2060.712232	21.141287
70.517789	2070.311532	21.146304
71.116943	2081.227606	21.151322
70.918229	2075.897287	21.156339
71.363385	2081.110127	21.161357
71.149776	2060.740325	21.166375
71.095885	2053.663086	21.171392
71.171090	2042.215516	21.176410
71.012912	2042.717134	21.181427
70.923393	2054.883486	21.186445
71.242558	2075.059609	21.191463
71.174102	2080.809391	21.196480
71.624888	2073.667165	21.201498
71.522544	2069.568095	21.206515
71.881934	2077.246013	21.211533
71.753919	2068.059005	21.216551
71.382057	2069.782769	21.221568
71.417652	2070.224230	21.226586
71.383910	2070.865407	21.231603
71.901639	2065.241216	21.236621
71.665441	2071.128717	21.241639
71.552382	2094.100755	21.246656
71.949017	2098.251568	21.251674
72.074198	2104.468005	21.256691
71.996777	2109.137772	21.261709
72.363208	2096.905135	21.266727
72.081273	2103.247501	21.271744
72.507048	2097.033846	21.276762
72.038563	2107.788394	21.281779
72.590852	2117.689431	21.286797
72.871375	2120.246133	21.291815
72.847158	2129.721327	21.296832
73.208237	2126.556660	21.301850
73.046464	2118.478797	21.306867
73.040949	2108.220994	21.311885
73.223812	2099.390182	21.316903
72.689300	2099.587411	21.321920
72.932761	2111.447676	21.326938
72.864218	2118.283727	21.331955
73.285492	2123.673388	21.336973
73.171183	2118.897935	21.341991
73.260999	2122.921397	21.347008
73.173742	2109.666493	21.352026
73.276533	2119.211519	21.357043
73.432323	2129.408779	21.362061
73.771834	2136.613643	21.367079
73.520252	2142.858852	21.372096
73.684579	2133.428334	21.377114
73.618437	2138.856093	21.382131
74.080191	2144.109504	21.387149
74.171859	2137.998212	21.392167
73.910087	2146.613667	21.397184
73.954844	2139.868425	21.402202
74.220531	2162.038627	21.407219
74.149690	2170.124715	21.412237
74.372208	2169.098862	21.417255
74.168263	2174.558591	21.422272
74.686930	2171.987029	21.427290
74.570342	2167.794630	21.432307
74.451987	2172.652719	21.437325
74.511280	2182.448326	21.442343
74.632341	2192.358872	21.447360
75.138878	2186.815241	21.452378
75.111120	2205.798769	21.457395
75.166468	2196.073325	21.462413
75.076772	2197.986040	21.467431
75.128699	2195.355821	21.472448
75.019454	2188.961751	21.477466
75.006441	2200.582419	21.482483
75.355581	2214.559109	21.487501
75.219823	2216.781457	21.492519
75.723031	2226.163936	21.497536
76.058667	2213.113471	21.502554
76.255606	2220.250335	21.507571
76.065632	2210.273914	21.512589
76.130076	2211.309418	21.517607
76.021223	2215.474980	21.522624
76.207444	2222.277791	21.527642
75.962437	2216.960629	21.532659
76.223986	2210.983283	21.537677
76.252583	2207.369514	21.542695
75.883225	2222.176268	21.547712
76.034345	2218.735840	21.552730
76.485022	2240.465164	21.557747
76.163371	2235.259161	21.562765
76.354207	2239.213107	21.567783
76.466106	2237.191434	21.572800
76.570961	2246.160196	21.577818
77.165057	2249.793576	21.582835
77.432844	2263.053889	21.587853
77.843748	2256.762720	21.592871
77.497740	2240.966778	21.597888
77.585895	2227.432220	21.602906
77.453822	2219.287950	21.607923
77.149973	2224.078849	21.612941
77.871783	2215.244625	21.617959
77.516472	2219.281065	21.622976
77.598945	2220.411607	21.627994
77.652513	2229.639283	21.633011
77.884550	2240.014894	21.638029
77.784162	2246.652351	21.643047
77.807728	2255.759435	21.648064
77.656937	2253.027066	21.653082
78.014285	2253.936727	21.658099
77.535259	2257.690579	21.663117
77.800382	2255.226893	21.668135
78.027868	2267.398996	21.673152
77.993683	2276.996019	21.678170
78.078141	2281.174748	21.683187
78.088570	2284.051176	21.688205
78.550119	2283.576946	21.693223
78.417756	2286.388915	21.698240
78.515921	2283.823440	21.703258
78.574312	2309.329974	21.708275
78.890244	2308.930340	21.713293
79.276434	2309.174167	21.718311
78.921178	2311.847587	21.723328
79.059830	2307.542256	21.728346
78.760673	2307.450757	21.733363
78.917892	2311.346134	21.738381
79.356977	2318.459335	21.743399
79.602434	2328.903250	21.748416
79.558651	2328.500403	21.753434
79.809754	2332.941224	21.758451
79.695803	2333.989848	21.763469
80.014775	2327.393447	21.768487
79.538763	2336.452104	21.773504
79.886218	2328.772982	21.778522
80.072378	2337.586153	21.783539
80.052229	2338.346345	21.788557
80.062190	2335.876626	21.793575
79.927983	2330.643376	21.798592
80.234327	2352.424798	21.803610
80.415432	2356.467009	21.808627
80.258732	2368.740050	21.813645
80.701962	2356.190106	21.818663
80.270111	2359.851100	21.823680
80.425705	2366.212986	21.828698
80.507149	2365.716489	21.833715
80.600573	2377.347554	21.838733
81.160498	2383.691071	21.843751
80.998154	2387.302950	21.848768
80.869712	2380.028101	21.853786
81.370980	2388.870039	21.858803
80.948292	2389.480589	21.863821
81.125595	2380.161943	21.868839
81.192689	2391.209579	21.873856
81.477621	2405.913673	21.878874
81.718026	2404.893101	21.883891
81.821616	2403.354695	21.888909
81.956193	2411.601264	21.893927
81.981970	2407.796966	21.898944
82.379041	2408.776022	21.903962
82.564626	2405.398725	21.908979
82.343095	2412.626485	21.913997
82.518590	2405.411352	21.919015
82.552761	2409.607135	21.924032
82.452889	2408.764772	21.929050
82.406885	2403.119580	21.934067
82.183002	2413.592732	21.939085
82.487087	2397.048802	21.944103
82.145647	2404.278769	21.949120
82.544627	2394.078361	21.954138
82.721628	2403.387992	21.959155
82.447830	2418.411342	21.964173
82.932775	2419.481704	21.969191
82.959827	2421.714820	21.974208
82.879273	2431.125936	21.979226
83.038626	2423.507557	21.984243
82.554412	2445.937050	21.989261
83.343495	2442.623628	21.994279
83.455824	2461.950342	21.999296
83.360516	2456.423565	22.004314
83.588772	2455.646751	22.009331
83.185473	2461.933443	22.014349
83.540634	2457.888951	22.019367
83.502429	2478.993137	22.024384
83.819926	2478.148732	22.029402
84.074229	2485.718722	22.034419
83.808847	2487.031116	22.039437
84.330619	2485.539351	22.044455
84.548372	2487.609675	22.049472
84.275666	2482.487584	22.054490
84.085993	2486.385535	22.059507
84.164104	2510.385122	22.064525
84.603482	2503.686744	22.069543
84.763344	2514.106424	22.074560
84.742753	2508.841239	22.079578
84.647141	2507.597358	22.084595
84.724010	2521.686113	22.089613
84.707370	2515.216278	22.094631
85.217762	2528.420358	22.099648
84.913921	2537.003252	22.104666
85.410834	2524.094237	22.109683
85.169824	2535.012856	22.114701
85.294843	2530.650671	22.119719
85.445924	2526.326678	22.124736
85.372030	2544.449743	22.129754
85.913225	2545.091062	22.134771
85.730313	2558.822613	22.139789
86.362530	2545.863139	22.144807
86.413809	2544.538935	22.149824
86.537752	2548.184772	22.154842
86.434517	2537.135409	22.159859
86.375633	2549.408084	22.164877
86.249290	2545.001839	22.169895
86.760457	2538.552157	22.174912
86.555204	2540.233713	22.179930
86.809324	2541.075111	22.184947
86.306761	2549.534339	22.189965
86.543103	2537.468654	22.194983
86.672250	2541.836492	22.200000
86.567841	2545.950613	22.205018
87.186119	2555.390552	22.210035
86.709668	2571.777712	22.215053
87.343746	2565.248140	22.220071
87.279797	2567.983825	22.225088
86.980807	2573.355546	22.230106
86.998550	2560.687560	22.235123
87.131676	2583.570585	22.240141
87.481667	2608.726379	22.245159
87.773087	2594.810460	22.250176
87.604742	2597.942652	22.255194
87.646524	2596.985000	22.260211
87.691122	2605.465535	22.265229
87.671160	2613.590643	22.270247
88.111593	2617.739044	22.275264
88.136004	2617.282335	22.280282
88.444464	2624.404788	22.285299
88.488653	2636.693081	22.290317
88.474893	2628.090722	22.295335
88.798386	2616.262080	22.300352
88.641827	2627.673054	22.305370
88.808401	2630.796839	22.310387
89.026745	2627.200653	22.315405
89.317300	2626.392610	22.320423
89.399080	2621.250538	22.325440
89.121023	2609.241939	22.330458
89.236784	2600.107021	22.335475
89.326705	2618.966765	22.340493
89.510922	2634.884333	22.345511
89.533534	2637.154046	22.350528
89.651801	2643.984085	22.355546
89.674335	2630.751437	22.360563
89.555928	2646.829158	22.365581
89.469878	2638.107698	22.370599
89.806335	2634.371797	22.375616
89.942822	2638.776633	22.380634
90.217801	2633.521343	22.385651
89.940794	2639.683568	22.390669
89.968552	2643.718267	22.395687
90.183084	2654.823875	22.400704
90.406178	2658.376091	22.405722
90.360639	2655.211176	22.410739
90.433993	2664.747256	22.415757
90.578997	2664.537053	22.420775
90.654862	2668.994889	22.425792
90.527367	2680.036090	22.430810
91.142885	2683.798306	22.435827
90.848333	2697.097326	22.440845
90.806694	2694.078614	22.445863
91.271408	2695.237797	22.450880
91.120232	2702.313833	22.455898
91.098669	2709.995532	22.460915
91.262991	2716.215552	22.465933
91.274839	2724.594501	22.470951
91.382511	2711.779549	22.475968
90.985776	2739.330648	22.480986
91.920829	2733.575840	22.486003
92.043616	2741.528857	22.491021
92.228618	2748.932137	22.496039
92.340441	2743.853146	22.501056
92.390792	2741.388068	22.506074
92.396306	2733.863613	22.511091
92.694958	2739.603024	22.516109
92.495628	2742.179338	22.521127
92.973827	2736.940243	22.526144
92.386471	2739.969254	22.531162
92.616008	2755.758147	22.536179
92.848173	2761.829108	22.541197
93.105638	2767.817515	22.546215
93.408312	2759.814896	22.551232
93.125318	2771.214307	22.556250
93.363873	2766.967054	22.561267
93.540881	2755.881592	22.566285
93.975056	2766.030644	22.571303
94.064551	2753.663587	22.576320
93.791654	2769.526544	22.581338
93.906603	2757.163523	22.586355
94.057327	2752.433991	22.591373
94.084305	2754.782134	22.596391
94.044916	2750.902750	22.601408
94.089988	2758.031634	22.606426
94.092149	2751.442429	22.611443
94.254099	2763.173818	22.616461
94.479261	2784.322056	22.621479
94.587741	2778.572308	22.626496
94.221706	2795.298459	22.631514
94.727368	2780.649483	22.636531
95.011420	2784.611309	22.641549
94.474358	2780.915812	22.646567
94.788162	2786.972428	22.651584
94.506410	2792.661457	22.656602
94.979439	2798.132919	22.661619
95.168843	2810.027509	22.666637
94.972220	2816.785931	22.671655
95.588719	2820.999623	22.676672
94.984764	2815.695053	22.681690
95.014382	2811.175406	22.686707
95.339052	2833.283612	22.691725
95.332069	2840.868458	22.696743
96.030474	2840.839136	22.701760
95.708974	2842.359322	22.706778
95.893027	2839.092825	22.711795
96.626871	2847.211686	22.716813
96.776498	2851.160433	22.721831
97.248654	2823.856714	22.726848
96.816752	2822.430884	22.731866
96.519363	2824.393153	22.736883
96.799158	2816.320681	22.741901
96.764940	2817.036774	22.746919
97.213408	2811.597071	22.751936
96.850457	2816.629089	22.756954
97.096344	2819.767686	22.761971
97.181356	2826.947448	22.766989
97.153894	2834.958556	22.772007
97.221258	2840.507295	22.777024
97.201071	2844.829166	22.782042
97.475303	2843.591908	22.787059
97.346847	2843.649211	22.792077
97.374382	2842.286011	22.797095
97.496677	2858.322767	22.802112
97.928792	2875.431748	22.807130
97.919930	2874.706920	22.812147
97.712635	2870.217178	22.817165
97.971996	2884.181833	22.822183
98.239485	2882.643704	22.827200
98.113207	2900.120332	22.832218
98.217886	2902.684341	22.837235
98.161025	2896.267886	22.842253
98.236108	2901.278713	22.847271
98.430214	2915.299125	22.852288
98.744824	2921.102099	22.857306
98.620780	2917.980100	22.862323
99.020560	2926.071051	22.867341
99.054436	2935.181937	22.872359
99.326348	2944.478483	22.877376
99.435931	2944.395038	22.882394
99.730173	2945.997957	22.887411
99.945152	2942.419978	22.892429
99.705962	2942.261415	22.897447
99.905814	2946.621948	22.902464
99.550252	2944.912928	22.907482
99.864953	2941.656589	22.912499
100.209109	2942.862208	22.917517
100.327285	2950.479855	22.922535
100.147591	2956.125208	22.927552
100.339600	2966.632377	22.932570
100.635217	2969.022923	22.937587
100.473463	2975.855940	22.942605
100.318928	2977.808660	22.947623
100.492791	2970.862457	22.952640
100.646290	2983.296255	22.957658
100.709540	2986.154586	22.962675
100.864766	2992.146291	22.967693
100.826547	2996.692083	22.972711
100.798324	2994.699112	22.977728
101.345923	3015.358220	22.982746
101.255610	3023.285374	22.987763
101.534204	3027.881289	22.992781
101.621397	3026.977880	22.997799
101.638577	3027.916955	23.002816
101.696943	3032.119516	23.007834
101.671347	3026.783722	23.012851
102.171427	3032.740181	23.017869
101.776949	3051.414788	23.022887
102.043182	3049.877639	23.027904
102.372616	3060.007674	23.032922
102.539510	3052.785011	23.037939
102.577812	3052.323224	23.042957
102.356599	3054.249631	23.047975
102.611905	3062.255599	23.052992
102.550995	3085.561797	23.058010
102.660956	3082.995019	23.063027
102.867766	3081.281507	23.068045
102.911405	3087.396919	23.073063
102.898380	3081.503067	23.078080
103.064884	3093.679654	23.083098
103.431682	3106.175749	23.088115
103.727645	3101.355828	23.093133
103.675054	3114.287405	23.098151
104.174230	3103.452907	23.103168
104.048595	3110.066183	23.108186
103.652974	3120.902627	23.113203
103.797709	3107.728800	23.118221
104.163848	3137.801674	23.123239
104.201459	3122.448603	23.128256
105.036581	3124.446340	23.133274
105.178381	3122.734572	23.138291
105.431656	3119.480137	23.143309
105.182279	3121.036398	23.148327
105.446230	3120.415052	23.153344
105.301403	3094.580832	23.158362
105.316883	3090.444981	23.163379
105.640421	3078.597478	23.168397
105.465108	3080.784392	23.173415
105.451391	3080.401333	23.178432
105.505757	3091.622461	23.183450
105.748141	3102.956851	23.188467
105.760345	3105.697299	23.193485
106.014385	3111.805710	23.198503
106.122622	3113.130085	23.203520
105.710241	3113.012507	23.208538
105.629316	3104.480106	23.213555
105.505197	3108.795305	23.218573
105.491744	3133.196533	23.223591
105.637649	3139.290640	23.228608
106.114231	3156.322456	23.233626
105.991512	3175.091036	23.238643
106.434343	3176.317682	23.243661
106.681365	3185.409435	23.248679
106.920823	3198.629978	23.253696
107.414439	3189.539805	23.258714
107.122502	3200.746902	23.263731
107.424674	3184.298137	23.268749
107.681649	3186.917993	23.273767
107.875847	3189.658528	23.278784
108.285768	3174.129744	23.283802
107.988447	3183.291091	23.288819
108.272684	3172.023327	23.293837
107.974917	3179.946845	23.298855
108.204591	3174.204373	23.303872
108.569007	3177.893080	23.308890
108.111456	3184.680061	23.313907
108.280111	3177.986622	23.318925
108.362319	3185.278837	23.323943
108.146332	3181.824790	23.328960
108.726112	3197.437019	23.333978
108.576092	3208.475643	23.338995
108.581829	3202.843611	23.344013
108.848962	3205.697236	23.349031
108.868432	3204.760185	23.354048
109.304901	3204.798810	23.359066
108.525559	3210.127729	23.364083
109.136329	3228.518549	23.369101
109.153579	3229.670636	23.374119
109.300888	3229.499024	23.379136
109.539643	3238.051977	23.384154
109.424299	3262.221105	23.389171
109.833638	3255.550239	23.394189
109.695307	3269.279728	23.399207
110.091893	3259.616609	23.404224
110.329071	3260.040748	23.409242
109.762415	3275.606546	23.414259
110.247072	3276.277774	23.419277
110.325991	3288.235189	23.424295
110.236309	3295.200475	23.429312
110.600886	3303.433707	23.434330
110.657065	3318.924392	23.439347
110.871432	3315.976017	23.444365
110.659800	3325.683496	23.449383
110.977329	3334.432092	23.454400
111.307944	3338.974569	23.459418
111.377632	3333.678746	23.464435
111.870347	3342.230894	23.469453
111.871813	3331.275783	23.474471
111.786373	3346.795149	23.479488
112.201845	3332.751651	23.484506
111.968626	3339.779003	23.489523
112.286553	3357.172479	23.494541
112.568084	3369.462069	23.499559
112.410266	3363.938269	23.504576
112.520390	3366.873140	23.509594
112.561828	3369.633582	23.514611
112.814838	3362.972113	23.519629
112.997170	3365.209877	23.524647
112.586358	3367.470615	23.529664
112.832858	3378.643876	23.534682
112.813189	3380.263179	23.539699
113.132792	3391.614871	23.544717
113.405786	3397.074512	23.549735
113.101741	3397.282661	23.554752
113.816606	3409.725489	23.559770
113.508259	3422.507284	23.564787
113.724121	3430.689700	23.569805
113.991529	3420.066747	23.574823
114.017668	3422.416312	23.579840
114.190577	3423.951643	23.584858
114.177765	3425.701714	23.589875
114.207061	3447.496851	23.594893
114.443091	3443.932191	23.599911
114.224807	3464.667988	23.604928
114.866915	3450.590659	23.609946
114.477726	3457.063608	23.614963
114.689691	3470.833890	23.619981
115.007755	3474.957188	23.624999
114.695684	3480.626303	23.630016
115.405712	3467.572821	23.635034
115.287822	3473.914856	23.640051
115.902161	3488.530192	23.645069
116.174011	3496.367869	23.650087
116.061678	3498.434520	23.655104
116.592300	3492.929746	23.660122
116.373446	3497.628943	23.665139
116.112712	3495.329236	23.670157
116.575485	3493.159714	23.675175
116.483678	3497.600765	23.680192
116.450230	3486.304066	23.685210
116.403695	3493.243370	23.690227
116.419689	3495.663144	23.695245
116.439694	3485.627776	23.700263
116.623571	3495.095598	23.705280
116.994069	3506.492859	23.710298
116.630323	3519.998190	23.715315
116.759785	3522.966495	23.720333
116.838056	3521.247917	23.725351
117.002121	3546.387302	23.730368
117.196865	3548.954169	23.735386
117.410972	3558.208715	23.740403
117.399150	3583.963675	23.745421
117.931345	3585.327491	23.750439
117.563073	3592.933761	23.755456
117.840659	3589.854738	23.760474
118.012731	3592.982136	23.765491
118.217707	3603.957318	23.770509
118.583463	3607.243499	23.775527
118.643285	3607.654991	23.780544
118.763392	3602.803112	23.785562
118.697825	3610.843000	23.790579
118.732105	3620.943308	23.795597
118.884151	3629.546323	23.800615
119.042889	3626.736285	23.805632
119.287492	3626.133099	23.810650
119.327877	3642.604401	23.815667
119.389959	3655.532723	23.820685
119.841478	3653.531999	23.825703
120.235525	3658.591650	23.830720
120.000860	3657.590100	23.835738
120.289914	3654.674926	23.840755
120.015851	3652.157305	23.845773
120.048712	3669.190581	23.850791
120.150111	3680.570083	23.855808
120.503674	3688.947100	23.860826
120.692944	3688.975228	23.865843
120.663237	3685.081009	23.870861
120.900688	3693.723810	23.875879
120.644741	3709.343925	23.880896
120.971331	3712.045228	23.885914
121.075868	3717.715282	23.890931
121.108744	3731.856541	23.895949
121.500575	3733.583896	23.900967
121.579526	3733.068478	23.905984
121.881387	3729.881050	23.911002
122.127237	3731.220804	23.916019
122.031394	3726.787891	23.921037
122.351038	3734.915420	23.926055
122.531477	3754.065075	23.931072
122.835556	3756.127921	23.936090
122.865959	3761.902448	23.941107
123.225097	3755.465334	23.946125
122.968249	3754.911613	23.951143
122.735524	3757.341653	23.956160
122.947358	3753.472245	23.961178
123.242055	3758.274783	23.966195
123.200593	3750.509976	23.971213
123.176744	3751.766975	23.976231
123.078378	3775.705305	23.981248
123.477291	3778.504457	23.986266
123.349635	3777.318953	23.991283
123.303749	3781.039372	23.996301
123.489620	3794.830420	24.001319
123.562256	3808.986798	24.006336
123.816762	3817.298446	24.011354
124.262278	3830.788864	24.016371
124.228033	3845.884021	24.021389
124.719989	3842.254692	24.026407
124.591318	3850.256364	24.031424
124.366422	3845.603100	24.036442
124.785097	3866.605673	24.041459
124.670185	3876.397037	24.046477
125.193121	3867.595737	24.051495
124.821322	3876.058746	24.056512
125.096484	3884.958019	24.061530
125.165464	3897.003784	24.066547
125.244409	3902.876609	24.071565
125.549188	3900.697852	24.076583
125.889435	3928.630994	24.081600
125.974253	3931.345738	24.086618
126.097452	3932.656672	24.091635
125.887057	3933.765528	24.096653
126.293851	3931.010683	24.101671
126.542937	3946.903455	24.106688
126.524260	3956.902923	24.111706
126.819625	3957.513897	24.116723
126.463144	3956.152992	24.121741
127.021142	3961.825348	24.126759
126.805459	3977.639853	24.131776
126.961639	3971.384037	24.136794
127.665017	3977.409456	24.141811
127.063282	3993.432639	24.146829
127.488577	3996.127039	24.151847
127.530014	4018.979762	24.156864
127.673235	4011.635773	24.161882
128.014666	4022.158198	24.166899
128.409493	4034.674402	24.171917
128.534376	4026.741244	24.176935
128.593383	4031.581459	24.181952
128.957471	4022.444608	24.186970
129.478482	4021.999047	24.191987
129.156897	4021.319047	24.197005
129.501904	4018.776846	24.202023
129.212957	4021.252494	24.207040
129.537289	4019.429184	24.212058
129.323566	4019.834956	24.217075
129.448596	4030.491395	24.222093
129.651999	4051.843420	24.227111
129.795927	4055.865086	24.232128
129.689468	4064.002171	24.237146
129.838359	4058.911083	24.242163
130.054748	4071.746775	24.247181
130.216248	4080.709149	24.252199
130.589183	4074.751571	24.257216
130.454127	4076.800023	24.262234
130.792124	4073.405312	24.267251
130.776799	4080.875199	24.272269
130.837148	4080.494377	24.277287
131.080569	4088.085073	24.282304
131.483341	4110.253383	24.287322
131.441737	4116.729083	24.292339
131.122157	4115.237997	24.297357
131.575270	4109.276139	24.302375
131.650337	4114.015665	24.307392
131.642063	4126.106337	24.312410
132.142953	4124.914402	24.317427
131.698886	4126.796462	24.322445
131.932308	4126.263237	24.327463
131.977897	4145.378292	24.332480
132.126315	4155.034717	24.337498
132.083514	4155.991704	24.342515
132.377414	4180.836475	24.347533
132.793412	4178.507289	24.352551
133.013144	4187.241511	24.357568
133.165620	4189.475694	24.362586
133.357323	4188.708419	24.367603
133.283568	4214.245932	24.372621
133.629492	4221.168378	24.377639
133.340348	4217.553790	24.382656
133.433404	4214.168646	24.387674
133.897705	4214.219981	24.392691
133.903324	4235.550786	24.397709
134.237514	4226.775140	24.402727
134.464064	4228.689099	24.407744
134.358636	4242.274186	24.412762
134.531098	4231.763724	24.417779
134.890357	4242.078974	24.422797
134.589510	4256.512421	24.427815
135.100122	4260.371614	24.432832
134.841562	4270.672997	24.437850
135.595382	4258.032521	24.442867
135.289521	4267.944850	24.447885
135.320780	4263.498933	24.452903
135.499559	4274.984531	24.457920
136.161555	4287.012770	24.462938
136.000340	4286.282875	24.467955
136.142414	4289.614249	24.472973
136.061244	4287.806318	24.477991
136.207108	4293.686283	24.483008
136.402351	4309.879362	24.488026
136.462821	4327.811664	24.493043
136.319956	4317.451199	24.498061
136.581461	4332.088163	24.503079
136.843934	4347.171507	24.508096
136.751251	4347.820995	24.513114
137.170200	4354.748692	24.518131
137.244313	4371.777844	24.523149
137.352548	4384.933783	24.528167
137.359937	4379.349093	24.533184
137.516666	4405.436113	24.538202
137.959518	4402.294425	24.543219
137.760226	4410.789692	24.548237
138.150776	4413.241868	24.553255
138.229685	4418.540783	24.558272
138.181434	4437.318973	24.563290
138.304500	4441.713557	24.568307
139.053726	4450.405614	24.573325
139.381796	4461.121533	24.578343
139.292687	4462.094108	24.583360
139.408121	4465.300004	24.588378
139.644968	4453.855705	24.593395
139.684395	4457.440433	24.598413
139.644961	4449.465459	24.603431
139.753933	4452.260545	24.608448
139.808196	4483.426201	24.613466
139.964258	4486.293797	24.618483
139.792774	4498.567811	24.623501
140.034988	4496.209181	24.628519
140.309618	4508.824099	24.633536
140.333738	4520.296989	24.638554
140.697426	4523.919989	24.643571
140.892372	4527.499365	24.648589
141.394564	4537.131102	24.653607
141.924024	4535.421704	24.658624
141.820788	4538.982906	24.663642
141.751978	4538.849559	24.668659
142.154924	4528.273823	24.673677
141.929725	4529.780916	24.678695
142.620024	4531.487905	24.683712
142.257784	4534.656638	24.688730
142.497119	4536.665377	24.693747
142.047719	4537.976617	24.698765
142.252206	4533.798739	24.703783
142.499685	4535.902205	24.708800
142.692165	4555.337503	24.713818
142.515009	4560.894803	24.718835
142.676691	4557.484794	24.723853
142.602076	4567.420312	24.728871
142.895314	4585.009449	24.733888
142.780051	4590.213107	24.738906
142.755215	4602.525835	24.743923
143.234885	4618.869642	24.748941
143.048291	4633.943620	24.753959
143.558362	4640.575150	24.758976
143.755773	4657.642401	24.763994
143.850363	4669.796728	24.769011
144.150408	4672.930248	24.774029
144.430634	4692.700805	24.779047
144.656412	4685.282536	24.784064
144.587115	4705.654598	24.789082
145.122981	4703.181773	24.794099
145.501015	4708.361775	24.799117
145.947719	4691.762592	24.804135
146.241890	4681.481258	24.809152
146.225585	4690.116377	24.814170
146.447523	4682.460909	24.819187
146.605380	4690.591410	24.824205
146.018551	4684.563525	24.829223
146.783420	4680.130252	24.834240
146.425870	4687.338341	24.839258
146.775071	4685.828205	24.844275
146.860668	4695.031539	24.849293
146.524726	4696.283773	24.854311
147.214193	4701.830994	24.859328
147.228282	4713.837286	24.864346
147.013610	4719.793074	24.869363
147.374515	4717.451703	24.874381
147.318255	4734.649398	24.879399
147.503737	4745.245086	24.884416
147.401567	4744.636089	24.889434
147.383430	4753.814956	24.894451
147.925460	4775.496808	24.899469
147.933395	4782.478033	24.904487
148.181041	4783.704962	24.909504
148.037170	4811.204282	24.914522
148.133441	4813.800719	24.919539
148.733333	4819.879502	24.924557
148.389379	4842.193806	24.929575
148.963282	4843.650044	24.934592
148.635046	4854.583977	24.939610
149.200076	4872.354300	24.944627
149.453419	4877.388117	24.949645
149.374281	4875.997971	24.954663
149.898916	4888.014063	24.959680
150.090903	4885.252619	24.964698
149.906757	4905.214805	24.969715
150.444067	4913.016960	24.974733
150.547790	4928.876999	24.979751
150.727999	4934.076561	24.984768
150.321972	4934.686785	24.989786
151.074270	4930.515428	24.994803
151.655444	4927.983063	24.999821
151.772620	4949.927920	25.004839
152.184405	4935.561501	25.009856
151.933078	4939.010366	25.014874
152.147321	4926.763809	25.019891
152.314243	4931.689933	25.024909
152.234054	4932.209784	25.029927
152.433255	4939.246714	25.034944
152.632813	4940.004387	25.039962
152.907598	4939.661942	25.044979
152.737267	4936.776408	25.049997
152.570748	4934.172974	25.055015
152.638238	4940.841163	25.060032
152.870659	4932.303343	25.065050
152.668381	4954.225686	25.070067
153.123615	4969.690280	25.075085
152.675469	4975.755054	25.080103
152.917150	4986.350230	25.085120
153.298693	4995.169061	25.090138
153.375433	5011.419573	25.095155
153.780344	5022.460185	25.100173
153.687706	5040.564442	25.105191
154.070920	5038.245308	25.110208
154.263289	5045.114095	25.115226
154.433353	5047.196630	25.120243
154.921610	5053.769745	25.125261
155.156502	5081.351508	25.130279
155.307981	5078.111622	25.135296
155.045699	5067.540536	25.140314
155.247255	5079.306463	25.145331
155.450090	5090.728019	25.150349
155.499216	5104.495296	25.155367
155.858484	5101.792650	25.160384
155.960216	5120.995645	25.165402
155.782489	5133.137302	25.170419
156.510876	5139.721742	25.175437
156.471506	5144.079724	25.180455
156.585301	5161.905670	25.185472
156.631792	5162.447006	25.190490
156.606300	5175.114697	25.195507
157.282620	5174.816571	25.200525
157.190740	5197.829017	25.205543
157.274425	5195.587986	25.210560
157.498528	5203.807767	25.215578
157.545721	5220.186264	25.220595
157.629629	5219.202946	25.225613
157.917324	5233.112621	25.230631
158.289842	5248.927529	25.235648
158.185389	5259.419742	25.240666
158.305816	5261.779118	25.245683
158.717574	5273.944214	25.250701
158.828315	5289.383673	25.255719
159.049957	5294.320508	25.260736
159.100381	5298.150899	25.265754
158.993641	5313.703704	25.270771
159.620038	5316.355471	25.275789
159.463799	5332.285893	25.280807
159.972515	5340.090651	25.285824
160.034420	5357.140226	25.290842
159.957640	5344.197444	25.295859
160.726273	5330.329763	25.300877
160.928286	5356.082415	25.305895
160.945142	5358.159736	25.310912
161.090594	5361.189135	25.315930
161.061112	5370.654563	25.320947
161.266089	5375.972231	25.325965
161.183611	5369.429462	25.330983
161.821139	5378.189433	25.336000
161.666567	5398.288306	25.341018
161.611396	5404.263526	25.346035
161.917754	5402.024843	25.351053
161.959667	5411.098817	25.356071
161.872886	5421.281044	25.361088
162.603480	5427.113887	25.366106
162.289264	5440.682720	25.371123
162.510111	5438.539363	25.376141
162.395085	5468.237117	25.381159
162.819800	5462.061315	25.386176
163.218642	5471.491856	25.391194
163.470861	5479.855175	25.396211
163.640877	5478.516508	25.401229
163.558120	5475.584031	25.406247
163.552206	5490.157827	25.411264
164.010289	5508.368002	25.416282
164.023458	5513.160766	25.421299
163.951187	5509.966637	25.426317
164.106051	5528.397340	25.431335
164.204302	5543.314591	25.436352
164.268100	5551.439115	25.441370
164.514100	5567.952694	25.446387
164.841203	5567.774814	25.451405
164.994667	5588.328374	25.456423
165.194295	5604.627597	25.461440
165.796200	5600.097504	25.466458
165.686518	5617.231004	25.471475
165.895777	5628.825942	25.476493
166.100309	5632.276390	25.481511
166.336589	5633.226470	25.486528
166.171999	5641.711117	25.491546
166.584297	5666.800835	25.496563
166.680863	5668.009623	25.501581
166.744030	5680.281791	25.506599
167.351150	5686.992942	25.511616
167.865023	5679.366455	25.516634
168.549419	5669.134627	25.521651
169.059807	5655.313515	25.526669
168.904357	5658.237817	25.531687
169.295696	5660.879875	25.536704
169.439494	5636.131975	25.541722
169.071748	5635.754519	25.546739
169.138347	5617.952656	25.551757
169.194327	5624.531687	25.556775
168.968981	5625.569501	25.561792
169.438575	5615.201706	25.566810
169.297281	5630.480182	25.571827
169.453407	5648.281530	25.576845
169.410309	5651.906234	25.581863
169.237307	5659.737011	25.586880
169.830199	5673.349845	25.591898
169.273845	5691.501187	25.596915
169.834101	5699.392861	25.601933
169.928882	5720.529715	25.606951
169.899504	5726.964665	25.611968
170.273730	5737.362689	25.616986
170.409415	5754.884806	25.622003
170.437784	5766.625682	25.627021
170.504065	5792.359071	25.632039
170.754220	5811.520917	25.637056
171.113264	5809.845223	25.642074
171.358285	5837.424264	25.647091
171.684626	5843.842683	25.652109
172.160176	5859.542636	25.657127
172.523699	5872.451046	25.662144
172.727179	5876.869689	25.667162
172.653166	5883.643702	25.672180
172.991074	5880.513656	25.677197
172.596265	5881.901775	25.682215
172.883972	5898.386718	25.687232
173.173650	5891.794494	25.692250
173.389813	5915.905128	25.697268
173.776975	5921.703865	25.702285
174.092700	5923.166096	25.707303
174.228845	5924.050134	25.712320
174.307845	5911.698485	25.717338
174.980022	5942.024786	25.722356
174.650839	5942.197753	25.727373
174.805133	5946.519049	25.732391
175.199617	5945.057196	25.737408
175.460650	5943.920746	25.742426
175.015176	5952.542808	25.747444
175.573788	5943.500518	25.752461
175.339206	5947.357948	25.757479
175.329043	5972.515203	25.762496
175.608506	5966.417689	25.767514
175.637685	5988.094287	25.772532
175.941937	5994.188793	25.777549
176.472118	6008.774012	25.782567
176.351903	6009.009132	25.787584
176.344294	6029.020588	25.792602
176.700155	6041.434215	25.797620
177.138130	6044.245015	25.802637
177.320607	6060.084443	25.807655
177.101479	6074.965146	25.812672
177.420369	6075.787323	25.817690
177.654366	6088.830851	25.822708
177.694904	6089.790645	25.827725
178.279641	6101.772480	25.832743
177.895332	6116.893327	25.837760
178.275162	6129.353448	25.842778
178.400367	6144.266788	25.847796
178.173176	6156.054355	25.852813
179.011587	6156.502729	25.857831
179.039912	6166.719079	25.862848
179.447014	6167.520302	25.867866
179.877412	6175.763021	25.872884
180.639376	6170.542999	25.877901
180.623627	6161.747249	25.882919
180.529076	6162.638918	25.887936
180.699089	6154.633791	25.892954
180.785258	6177.349499	25.897972
180.759023	6188.905219	25.902989
181.299607	6194.769929	25.908007
180.979701	6198.729023	25.913024
181.246899	6198.151531	25.918042
181.575860	6214.982805	25.923060
181.465883	6223.299588	25.928077
181.700222	6226.585328	25.933095
181.916230	6241.061505	25.938112
182.264142	6260.754264	25.943130
182.140874	6248.703754	25.948148
181.965375	6273.056441	25.953165
182.103690	6281.825051	25.958183
182.150933	6305.476808	25.963200
183.063571	6313.727683	25.968218
183.127511	6318.140495	25.973236
183.291602	6336.970724	25.978253
183.828518	6337.242367	25.983271
183.508737	6350.253685	25.988288
184.119081	6358.232674	25.993306
184.140338	6367.995866	25.998324
184.080088	6374.958408	26.003341
184.656773	6380.358789	26.008359
184.636541	6395.895919	26.013376
184.783370	6399.423074	26.018394
184.790086	6406.979402	26.023412
185.193012	6434.701014	26.028429
185.363570	6436.560754	26.033447
185.879958	6447.055347	26.038464
185.895584	6458.334937	26.043482
185.736101	6473.085594	26.048500
185.919586	6474.655704	26.053517
186.504241	6487.126970	26.058535
186.690985	6498.111146	26.063552
186.536285	6496.525475	26.068570
186.827125	6509.417344	26.073588
187.000348	6508.357670	26.078605
187.263467	6519.877366	26.083623
187.043093	6530.087229	26.088640
187.171233	6528.925564	26.093658
187.286338	6555.006518	26.098676
187.148728	6571.061111	26.103693
187.568410	6582.812396	26.108711
187.571284	6597.784296	26.113728
187.843864	6614.904190	26.118746
188.064136	6631.065569	26.123764
188.080686	6655.935918	26.128781
188.905480	6661.464514	26.133799
189.040739	6682.367510	26.138816
189.400875	6685.635594	26.143834
190.099761	6692.173616	26.148852
190.108692	6698.448217	26.153869
190.859570	6698.295220	26.158887
190.261054	6704.952735	26.163904
190.901927	6703.871266	26.168922
191.268607	6704.884813	26.173940
190.926884	6709.019363	26.178957
191.183128	6727.934777	26.183975
191.442127	6733.267559	26.188992
191.647037	6721.042436	26.194010
192.040796	6719.462489	26.199028
191.861164	6747.032551	26.204045
192.087180	6751.629643	26.209063
192.343523	6753.494071	26.214080
192.249113	6752.885279	26.219098
192.396465	6768.866730	26.224116
192.633916	6776.710194	26.229133
193.178393	6765.412388	26.234151
193.490120	6784.628984	26.239168
193.661803	6796.438965	26.244186
194.044445	6785.078244	26.249204
194.184933	6799.660424	26.254221
194.477858	6786.448666	26.259239
194.272415	6795.552720	26.264256
194.471038	6811.358713	26.269274
194.785458	6815.815110	26.274292
195.094344	6824.669888	26.279309
194.840319	6820.785779	26.284327
195.247218	6839.655027	26.289344
195.560566	6852.276422	26.294362
195.501645	6843.025902	26.299380
195.492288	6863.773582	26.304397
195.951174	6869.742703	26.309415
196.056682	6880.553970	26.314432
196.274113	6877.593406	26.319450
196.433956	6897.937305	26.324468
196.513345	6909.411412	26.329485
196.953593	6912.047135	26.334503
196.967149	6931.886868	26.339520
197.157863	6934.483717	26.344538
197.547315	6946.146565	26.349556
197.273572	6966.073462	26.354573
197.395807	6971.794523	26.359591
197.754851	6981.848537	26.364608
197.617798	7009.006334	26.369626
198.093897	7013.782494	26.374644
198.086731	7036.792199	26.379661
198.484295	7057.537894	26.384679
198.688507	7069.827874	26.389696
198.808899	7075.473664	26.394714
199.301300	7083.781387	26.399732
199.156359	7109.492938	26.404749
199.745393	7121.461449	26.409767
199.719564	7133.835388	26.414784
199.971833	7137.104949	26.419802
200.406178	7147.103235	26.424820
200.022033	7155.201404	26.429837
200.605006	7149.086091	26.434855
201.060029	7164.756888	26.439872
201.537326	7179.533145	26.444890
201.853538	7184.484006	26.449908
201.888540	7175.181454	26.454925
202.033077	7179.492108	26.459943
202.326974	7198.958710	26.464960
202.671916	7205.036686	26.469978
202.811942	7205.339641	26.474996
202.718699	7214.596216	26.480013
202.815716	7201.439509	26.485031
203.051136	7217.964450	26.490048
203.112841	7236.780467	26.495066
203.365564	7225.655268	26.500084
203.079373	7246.247014	26.505101
203.304748	7251.199600	26.510119
203.660570	7274.925982	26.515136
203.909255	7302.455769	26.520154
204.033398	7305.932547	26.525172
203.985860	7327.752902	26.530189
204.204698	7343.250448	26.535207
204.747959	7361.124090	26.540224
204.639535	7375.837955	26.545242
205.062572	7385.604330	26.550260
205.235195	7417.220834	26.555277
205.596418	7430.856358	26.560295
206.038660	7435.291694	26.565312
205.945378	7463.105432	26.570330
206.539558	7459.976612	26.575348
206.480193	7481.056357	26.580365
206.544292	7489.230663	26.585383
207.315294	7499.848279	26.590400
207.496054	7512.440245	26.595418
208.100133	7526.538831	26.600436
207.871375	7521.820915	26.605453
208.107603	7524.693867	26.610471
208.124323	7549.311951	26.615488
208.567393	7538.466831	26.620506
209.000569	7538.309911	26.625524
209.081479	7569.977404	26.630541
209.246068	7570.232963	26.635559
209.719682	7563.513391	26.640576
209.477980	7568.514540	26.645594
209.998813	7574.462610	26.650612
210.076737	7604.116547	26.655629
209.755184	7612.400681	26.660647
210.173475	7609.760282	26.665664
210.184299	7632.307848	26.670682
210.389141	7642.230366	26.675700
210.839807	7666.616627	26.680717
210.899054	7665.556913	26.685735
210.610851	7679.131204	26.690752
210.926712	7699.792066	26.695770
211.399350	7713.537716	26.700788
211.832651	7731.702591	26.705805
211.661297	7740.162697	26.710823
211.918621	7745.849777	26.715840
212.256465	7775.312757	26.720858
212.569552	7781.203263	26.725876
212.705916	7798.709411	26.730893
212.776157	7811.297133	26.735911
213.559095	7824.288692	26.740928
213.266808	7844.202436	26.745946
213.674432	7841.470035	26.750964
214.253771	7851.779450	26.755981
214.309757	7859.011626	26.760999
214.683861	7865.442629	26.766016
214.595487	7876.403369	26.771034
214.868451	7873.233319	26.776052
215.254038	7890.817889	26.781069
215.221692	7902.376658	26.786087
215.174963	7909.253339	26.791104
215.487154	7927.673297	26.796122
215.872247	7936.278937	26.801140
216.009858	7952.219873	26.806157
216.177333	7964.540282	26.811175
216.440464	7962.715679	26.816192
216.347820	7979.985955	26.821210
216.998247	7988.027648	26.826228
217.352246	7998.611700	26.831245
217.347733	8024.462087	26.836263
217.869828	8034.916619	26.841280
217.710590	8030.112955	26.846298
217.664374	8037.804887	26.851316
218.127512	8047.472059	26.856333
218.405906	8084.891147	26.861351
218.848418	8089.447144	26.866368
218.911846	8090.191362	26.871386
219.351206	8105.109487	26.876404
219.387202	8123.332947	26.881421
219.140083	8122.166564	26.886439
219.578385	8137.092772	26.891456
219.613355	8157.827684	26.896474
219.576747	8168.666591	26.901492
220.299992	8192.720852	26.906509
220.324322	8210.437483	26.911527
220.894022	8212.577714	26.916544
221.473180	8229.260065	26.921562
221.639250	8233.669833	26.926580
222.068333	8229.079507	26.931597
222.116949	8262.795515	26.936615
222.727024	8252.896579	26.941632
222.510416	8257.332914	26.946650
222.651805	8261.656990	26.951668
222.669435	8280.435087	26.956685
223.054179	8284.331175	26.961703
223.515048	8297.140320	26.966720
223.670894	8316.088487	26.971738
223.933004	8323.164528	26.976756
224.397661	8314.607582	26.981773
224.429033	8321.657367	26.986791
224.584858	8337.286873	26.991808
224.327047	8343.536335	26.996826
224.772517	8359.266618	27.001844
225.151878	8368.934516	27.006861
225.367053	8375.511869	27.011879
225.590073	8385.036391	27.016896
225.726247	8401.731085	27.021914
225.728279	8414.315650	27.026932
226.012151	8419.847318	27.031949
226.242907	8438.547652	27.036967
226.410025	8446.321707	27.041984
226.478580	8473.596715	27.047002
226.782837	8478.709880	27.052020
226.939872	8499.370600	27.057037
226.966172	8518.251518	27.062055
227.314644	8535.171030	27.067072
227.742630	8556.669069	27.072090
227.786134	8576.759525	27.077108
228.031482	8581.489430	27.082125
228.021222	8609.348088	27.087143
228.766409	8623.343858	27.092160
229.036786	8641.513999	27.097178
229.072971	8651.640048	27.102196
229.431682	8650.660491	27.107213
229.396415	8675.574113	27.112231
229.995708	8674.077208	27.117248
230.005152	8691.063457	27.122266
230.220081	8702.647888	27.127284
230.421804	8708.083022	27.132301
230.568173	8721.620650	27.137319
230.862680	8725.886326	27.142336
230.932265	8743.469202	27.147354
230.893627	8753.233569	27.152372
231.341894	8768.900773	27.157389
231.041511	8792.581686	27.162407
231.337058	8808.352291	27.167424
231.684507	8840.553863	27.172442
232.086575	8854.762034	27.177460
232.233383	8881.514272	27.182477
232.699354	8908.486876	27.187495
233.362348	8911.782309	27.192512
233.922585	8929.604483	27.197530
233.927225	8942.705010	27.202548
234.909230	8934.339857	27.207565
234.764523	8949.127369	27.212583
235.203688	8951.644671	27.217600
235.086535	8974.291807	27.222618
235.476894	8975.467006	27.227636
235.576827	8973.231413	27.232653
235.641727	8978.932790	27.237671
235.848435	8995.967726	27.242688
236.040795	9007.144918	27.247706
235.610032	9027.050839	27.252724
235.915650	9035.711246	27.257741
236.340965	9059.057706	27.262759
236.938178	9073.192686	27.267776
236.895477	9094.694030	27.272794
237.154730	9103.419683	27.277812
237.683923	9121.400057	27.282829
237.926482	9130.059963	27.287847
238.410084	9141.031307	27.292864
238.295871	9153.478213	27.297882
238.589942	9165.764336	27.302900
238.977488	9184.134627	27.307917
239.035906	9192.003520	27.312935
239.178232	9203.543659	27.317952
239.574856	9217.254401	27.322970
239.795675	9227.273724	27.327988
240.053761	9251.972494	27.333005
240.268297	9262.258362	27.338023
240.729085	9271.755726	27.343040
240.687945	9293.921170	27.348058
240.772209	9309.847904	27.353076
241.052351	9327.930549	27.358093
241.272712	9333.541624	27.363111
241.577318	9346.782496	27.368128
241.679993	9370.706102	27.373146
241.887577	9369.995037	27.378164
242.017664	9402.155865	27.383181
242.120490	9418.993447	27.388199
242.397385	9449.496122	27.393216
242.814465	9462.853901	27.398234
242.936256	9487.487447	27.403252
243.469542	9504.559258	27.408269
243.252968	9516.400316	27.413287
243.911917	9545.510703	27.418304
243.765199	9553.921190	27.423322
244.193498	9580.435606	27.428340
244.587021	9577.646967	27.433357
244.773221	9611.733697	27.438375
244.946043	9627.166269	27.443392
245.378252	9638.349744	27.448410
245.619921	9652.044852	27.453428
245.919989	9659.411390	27.458445
246.058921	9678.655464	27.463463
246.713987	9697.553834	27.468480
247.160704	9706.065903	27.473498
246.716380	9720.472980	27.478516
247.083536	9725.738384	27.483533
247.305303	9739.281678	27.488551
247.570356	9744.509694	27.493568
247.617329	9761.748450	27.498586
247.740811	9772.658742	27.503604
248.331321	9790.312199	27.508621
248.054742	9813.136686	27.513639
248.289171	9836.212693	27.518656
249.110343	9850.877582	27.523674
248.911648	9869.916430	27.528692
249.767968	9882.539041	27.533709
249.912701	9908.633158	27.538727
250.324317	9918.175317	27.543744
250.471765	9930.105879	27.548762
250.865324	9942.601383	27.553780
251.237930	9953.023720	27.558797
251.470488	9969.210080	27.563815
251.792578	9982.790482	27.568832
251.994042	9993.125472	27.573850
251.900856	10008.159071	27.578868
252.623195	10009.397365	27.583885
253.047802	10020.004120	27.588903
253.145190	10033.287079	27.593920
253.538100	10028.428890	27.598938
253.814609	10040.562617	27.603956
254.431447	10054.095685	27.608973
254.480384	10066.766714	27.613991
254.334960	10063.790228	27.619008
254.809396	10063.995928	27.624026
254.986983	10076.533722	27.629044
255.334211	10082.346934	27.634061
255.441873	10092.987489	27.639079
255.715724	10096.551875	27.644096
255.712341	10119.895479	27.649114
255.810264	10128.220714	27.654132
255.993175	10147.211457	27.659149
255.985627	10173.356515	27.664167
256.057001	10185.214823	27.669184
257.003853	10199.680319	27.674202
256.837550	10217.329211	27.679220
257.289243	10219.299469	27.684237
257.344222	10243.875159	27.689255
257.292570	10276.858904	27.694272
258.403012	10284.533061	27.699290
258.297013	10303.659437	27.704308
258.574015	10310.113871	27.709325
258.706991	10327.870725	27.714343
259.266015	10340.325656	27.719360
259.491618	10357.654334	27.724378
259.267556	10384.797643	27.729396
259.649885	10400.300930	27.734413
260.223348	10409.868491	27.739431
260.441864	10444.477100	27.744448
260.767339	10434.928225	27.749466
260.580768	10469.081071	27.754484
261.114506	10487.152040	27.759501
261.504111	10507.112564	27.764519
261.590366	10516.370370	27.769536
261.881895	10530.657485	27.774554
262.146969	10545.621820	27.779572
262.593810	10572.834393	27.784589
262.880598	10574.843912	27.789607
262.846940	10590.294382	27.794624
263.364708	10588.379915	27.799642
263.150531	10621.439424	27.804660
263.360416	10641.691537	27.809677
263.762215	10656.585989	27.814695
264.157750	10678.420801	27.819712
264.604833	10683.099696	27.824730
264.614620	10709.464127	27.829748
265.097565	10721.072457	27.834765
265.524765	10729.556015	27.839783
265.228378	10746.933232	27.844800
265.940575	10749.906535	27.849818
266.273697	10775.851795	27.854836
266.663405	10795.357286	27.859853
266.802232	10806.652563	27.864871
266.929733	10816.920800	27.869888
267.253492	10828.976367	27.874906
267.211676	10857.264085	27.879924
267.554838	10871.992001	27.884941
267.754541	10891.885284	27.889959
268.044803	10910.660553	27.894976
268.220946	10934.024356	27.899994
268.624067	10942.148038	27.905012
268.645054	10969.253190	27.910029
269.321164	10983.049796	27.915047
269.341111	11005.190112	27.920064
269.560659	11023.099587	27.925082
269.958099	11047.813419	27.930100
270.443656	11065.221787	27.935117
270.948384	11081.505075	27.940135
271.199645	11094.924857	27.945152
271.878448	11091.414947	27.950170
272.517841	11105.020792	27.955188
272.653250	11099.325814	27.960205
273.060064	11110.167093	27.965223
272.830725	11132.675175	27.970240
273.324868	11138.043645	27.975258
273.489131	11138.730285	27.980276
273.320790	11161.039186	27.985293
273.833544	11173.471726	27.990311
273.232179	11194.204400	27.995328
273.805809	11208.856517	28.000346
274.311805	11235.520693	28.005364
274.276425	11249.747732	28.010381
274.193675	11272.247411	28.015399
274.756502	11296.570151	28.020416
275.272586	11308.274249	28.025434
275.726680	11335.402604	28.030452
275.840385	11353.821665	28.035469
276.432783	11366.855665	28.040487
276.356917	11390.410117	28.045504
276.915032	11403.854812	28.050522
277.157625	11432.655677	28.055540
277.029001	11441.849653	28.060557
277.384643	11462.111671	28.065575
277.421370	11493.932912	28.070592
278.052730	11510.647840	28.075610
278.100978	11532.352417	28.080628
278.603545	11558.010782	28.085645
278.994567	11569.505786	28.090663
279.187601	11587.878842	28.095680
279.322440	11599.329762	28.100698
280.142550	11622.541876	28.105716
280.054640	11634.187405	28.110733
280.676529	11648.195291	28.115751
280.733743	11674.985179	28.120768
281.170230	11670.894550	28.125786
281.086733	11686.543440	28.130804
281.214626	11702.776508	28.135821
281.655607	11711.984733	28.140839
281.709125	11736.874942	28.145856
282.172487	11751.107805	28.150874
282.375982	11767.199162	28.155892
282.213920	11791.788053	28.160909
282.583756	11820.877324	28.165927
282.310173	11836.526423	28.170944
282.956339	11866.898264	28.175962
283.358823	11894.073951	28.180980
283.365881	11924.736449	28.185997
283.923829	11953.789979	28.191015
284.248779	11979.410763	28.196032
285.058907	11994.807482	28.201050
286.154356	12006.176313	28.206068
286.628713	12015.735300	28.211085
286.968045	12018.616367	28.216103
286.957928	12018.657569	28.221120
287.543063	12021.696351	28.226138
287.704547	12041.454001	28.231156
287.459108	12051.947291	28.236173
288.177085	12049.658236	28.241191
288.412685	12058.286213	28.246208
288.597646	12081.886581	28.251226
288.438985	12086.793380	28.256244
288.560399	12098.492712	28.261261
289.144642	12115.176702	28.266279
288.967195	12146.790553	28.271296
289.430573	12152.254300	28.276314
289.904807	12171.109202	28.281332
289.595172	12204.346168	28.286349
290.091285	12218.135921	28.291367
290.109392	12243.070610	28.296384
290.289250	12267.545109	28.301402
290.935370	12298.035956	28.306420
291.356131	12317.813901	28.311437
291.654862	12331.483687	28.316455
291.609391	12362.113190	28.321472
291.717050	12383.487562	28.326490
292.313575	12406.952266	28.331508
292.421780	12445.689364	28.336525
292.713913	12454.998385	28.341543
293.136984	12493.464243	28.346560
293.506101	12520.490514	28.351578
294.026999	12547.490039	28.356596
294.163618	12563.443591	28.361613
294.749580	12578.830836	28.366631
294.832037	12606.478490	28.371648
295.430395	12617.290538	28.376666
295.735873	12635.110305	28.381684
296.320196	12657.297791	28.386701
296.624562	12662.603752	28.391719
296.965252	12680.212854	28.396736
297.021580	12693.516640	28.401754
297.321384	12703.341418	28.406772
297.390189	12732.687202	28.411789
297.853199	12735.232675	28.416807
298.019180	12768.300373	28.421824
298.288618	12783.765613	28.426842
298.583578	12801.094057	28.431860
298.695102	12815.501350	28.436877
299.182817	12841.101183	28.441895
299.400847	12861.693539	28.446912
299.698083	12885.629423	28.451930
300.053615	12909.645484	28.456948
300.152550	12932.278019	28.461965
300.299683	12938.533671	28.466983
301.005081	12956.985476	28.472000
301.264891	12998.215422	28.477018
301.622215	12990.637529	28.482036
301.871616	13017.640391	28.487053
302.190266	13025.575869	28.492071
302.680841	13044.304577	28.497088
302.504366	13057.670976	28.502106
302.747303	13077.873369	28.507124
302.781729	13110.002307	28.512141
303.132898	13124.042270	28.517159
303.482638	13159.398413	28.522176
303.518057	13189.065750	28.527194
304.852247	13188.536919	28.532212
305.351818	13195.083975	28.537229
306.003897	13205.148384	28.542247
306.430430	13220.868457	28.547264
306.418790	13232.631685	28.552282
306.579386	13229.828341	28.557300
306.804856	13248.577688	28.562317
307.060463	13260.444675	28.567335
307.113312	13282.217013	28.572352
307.285488	13299.051055	28.577370
308.109513	13308.726074	28.582388
307.388291	13336.607767	28.587405
307.908088	13355.130259	28.592423
308.467016	13390.329228	28.597440
308.428924	13405.625518	28.602458
309.167139	13430.262735	28.607476
309.495807	13450.489171	28.612493
309.928051	13470.337532	28.617511
310.595726	13493.026076	28.622528
310.407439	13501.934845	28.627546
310.797749	13523.084097	28.632564
311.031006	13547.439757	28.637581
311.312354	13570.107488	28.642599
311.427713	13587.017456	28.647616
311.911408	13613.820060	28.652634
312.323542	13638.773375	28.657652
312.166127	13659.312491	28.662669
312.589713	13683.354636	28.667687
313.131537	13710.021662	28.672704
312.927866	13747.500877	28.677722
313.489253	13765.914490	28.682740
313.718021	13804.100529	28.687757
314.371605	13829.489972	28.692775
314.256419	13844.931862	28.697792
314.795714	13864.747160	28.702810
315.478836	13893.266443	28.707828
315.418709	13917.529556	28.712845
315.754837	13943.071202	28.717863
315.990400	13963.625790	28.722880
316.177308	13994.382079	28.727898
316.910074	14016.316666	28.732916
317.159614	14050.807248	28.737933
317.301146	14071.957565	28.742951
317.558052	14095.927143	28.747968
318.101339	14120.563117	28.752986
318.673260	14139.640481	28.758004
318.672317	14177.648063	28.763021
319.088212	14191.503256	28.768039
319.519476	14211.600119	28.773056
319.861732	14241.913419	28.778074
320.257431	14262.115542	28.783092
320.432657	14279.459145	28.788109
320.538111	14311.865484	28.793127
321.035489	14324.681255	28.798144
321.467406	14353.213130	28.803162
321.725335	14361.597489	28.808180
321.844256	14389.721221	28.813197
322.122312	14412.140076	28.818215
322.483726	14426.203101	28.823232
322.641916	14456.753840	28.828250
322.947340	14468.829350	28.833268
323.549388	14494.954950	28.838285
323.596084	14513.292578	28.843303
323.923128	14539.854797	28.848320
324.589658	14564.526128	28.853338
324.838916	14593.238492	28.858356
325.524628	14609.917651	28.863373
325.604088	14623.780244	28.868391
326.207534	14642.057047	28.873408
326.351780	14669.162065	28.878426
327.010732	14679.473695	28.883444
327.006804	14704.768841	28.888461
327.309284	14723.073668	28.893479
327.885277	14737.627724	28.898496
327.767121	14769.047664	28.903514
328.166169	14781.333231	28.908532
328.588424	14806.976973	28.913549
328.528706	14827.422515	28.918567
329.062071	14847.676568	28.923584
329.281095	14892.522576	28.928602
329.647285	14911.504206	28.933620
329.814213	14935.210992	28.938637
330.242468	14965.815532	28.943655
330.623942	14980.635381	28.948672
330.608507	15012.513127	28.953690
331.237231	15045.027846	28.958708
331.601570	15065.863461	28.963725
332.116866	15097.070044	28.968743
332.216666	15132.312788	28.973760
332.359433	15160.868887	28.978778
332.861605	15178.767510	28.983796
333.502853	15218.018397	28.988813
333.570051	15244.560302	28.993831
334.071514	15269.442950	28.998848
334.131124	15300.938398	29.003866
334.621878	15320.661078	29.008884
334.970601	15351.921036	29.013901
335.485373	15372.446770	29.018919
336.073865	15403.381714	29.023936
336.111478	15430.061229	29.028954
336.718546	15451.528448	29.033972
336.877528	15473.878695	29.038989
337.314501	15493.539591	29.044007
337.979229	15500.115313	29.049024
337.956318	15527.038310	29.054042
338.320593	15545.600159	29.059060
338.720396	15569.070578	29.064077
339.092037	15588.444548	29.069095
339.628996	15616.554525	29.074112
339.510843	15631.201048	29.079130
340.127460	15654.500022	29.084148
340.683203	15679.694236	29.089165
341.022930	15702.098305	29.094183
341.349249	15719.599590	29.099200
341.393359	15746.333704	29.104218
341.973022	15772.800787	29.109236
342.142037	15785.226198	29.114253
341.923596	15811.037836	29.119271
342.655954	15844.145328	29.124288
342.589914	15883.261534	29.129306
342.922571	15900.103113	29.134324
343.344486	15923.130609	29.139341
343.770579	15954.832802	29.144359
343.960347	15981.308247	29.149376
343.843507	16005.293839	29.154394
344.332254	16034.807474	29.159412
344.702090	16051.349858	29.164429
345.003440	16089.614269	29.169447
345.778940	16111.487828	29.174464
345.938316	16143.631896	29.179482
346.436216	16176.047642	29.184500
346.945243	16195.437334	29.189517
346.903730	16241.766228	29.194535
347.453470	16266.992288	29.199552
347.490014	16295.456087	29.204570
348.316282	16316.886448	29.209588
348.478402	16348.868107	29.214605
348.750427	16374.589691	29.219623
349.211578	16400.765377	29.224640
349.545773	16432.855746	29.229658
349.701948	16461.875285	29.234676
350.256373	16494.225523	29.239693
350.745865	16530.301824	29.244711
351.076861	16554.316273	29.249728
351.803615	16588.155996	29.254746
352.173203	16602.545815	29.259764
352.456216	16618.333981	29.264781
352.521210	16649.985581	29.269799
352.991370	16667.156608	29.274816
353.240321	16696.883075	29.279834
353.617559	16722.036030	29.284852
354.161535	16750.923876	29.289869
354.364487	16786.337439	29.294887
354.668210	16802.199577	29.299904
354.912245	16830.759083	29.304922
355.705629	16865.515157	29.309940
355.976336	16883.037950	29.314957
356.189225	16914.733268	29.319975
356.700869	16936.270296	29.324992
357.175612	16956.891354	29.330010
357.629699	16987.421275	29.335028
357.992568	17000.677629	29.340045
358.164702	17040.489980	29.345063
358.743261	17063.934411	29.350080
359.093485	17077.040026	29.355098
359.495243	17104.013267	29.360116
359.922657	17119.732212	29.365133
360.052444	17154.427312	29.370151
360.676255	17168.384471	29.375168
360.707339	17181.820613	29.380186
360.788926	17213.241968	29.385204
361.442699	17231.931021	29.390221
361.732510	17265.061287	29.395239
361.723199	17289.576280	29.400256
362.196021	17326.380618	29.405274
362.321980	17354.109426	29.410292
362.990322	17375.956755	29.415309
363.064823	17422.427310	29.420327
363.133389	17447.558555	29.425344
363.668738	17492.119474	29.430362
363.803475	17533.209748	29.435380
364.481737	17557.916730	29.440397
364.699230	17594.787723	29.445415
365.183150	17629.956218	29.450432
365.507181	17669.678639	29.455450
365.931345	17704.713770	29.460468
366.618982	17727.682303	29.465485
366.324161	17762.375115	29.470503
366.802318	17799.578437	29.475520
367.311735	17829.810667	29.480538
367.661160	17861.395259	29.485556
368.207184	17894.916147	29.490573
368.587907	17933.840017	29.495591
368.586500	17947.018920	29.500608
369.457234	17988.725807	29.505626
369.442388	18009.814142	29.510644
370.158369	18034.559709	29.515661
370.347139	18072.177434	29.520679
370.695376	18096.154998	29.525696
371.282329	18138.719669	29.530714
371.494761	18166.670351	29.535732
371.916318	18194.026717	29.540749
372.218127	18225.771246	29.545767
372.532746	18258.383886	29.550784
373.146103	18289.849782	29.555802
373.435994	18314.910891	29.560820
373.871332	18341.191671	29.565837
374.023295	18375.833612	29.570855
374.302808	18401.293833	29.575872
375.031946	18445.093656	29.580890
375.413169	18474.506541	29.585908
375.952474	18504.835926	29.590925
375.814132	18546.043423	29.595943
376.374812	18572.089352	29.600960
377.194554	18594.212663	29.605978
377.205565	18635.673026	29.610996
377.441679	18658.886531	29.616013
377.734113	18714.751653	29.621031
378.159156	18735.893952	29.626048
378.531985	18767.659244	29.631066
378.668307	18816.108176	29.636084
379.280880	18860.612639	29.641101
379.714020	18879.233003	29.646119
379.917605	18917.890644	29.651136
380.445081	18957.866107	29.656154
380.417834	19006.044805	29.661172
381.112565	19017.721614	29.666189
381.748522	19072.791499	29.671207
381.782564	19113.046359	29.676224
382.302554	19146.651341	29.681242
382.500343	19192.980228	29.686260
382.870873	19226.328003	29.691277
383.516509	19276.003738	29.696295
384.093919	19312.506594	29.701312
384.633322	19336.985472	29.706330
384.725897	19376.687345	29.711348
385.519645	19410.480709	29.716365
385.578581	19442.556398	29.721383
386.396623	19473.873867	29.726400
386.695709	19503.880794	29.731418
387.024980	19546.909642	29.736436
387.699499	19571.530380	29.741453
387.662474	19601.793533	29.746471
388.120203	19626.940666	29.751488
388.634177	19657.238518	29.756506
389.007824	19698.817848	29.761524
389.199048	19714.394027	29.766541
389.436168	19754.952500	29.771559
390.039442	19787.584816	29.776576
390.632317	19818.254532	29.781594
390.875580	19857.011803	29.786612
391.478946	19884.884656	29.791629
391.616754	19917.690713	29.796647
391.616843	19949.838633	29.801664
392.190607	19977.699215	29.806682
392.514924	20025.857129	29.811700
393.000786	20059.013982	29.816717
393.445592	20095.620979	29.821735
393.793292	20124.001790	29.826752
394.298238	20151.560352	29.831770
394.419615	20191.063870	29.836788
394.907675	20217.066095	29.841805
395.368671	20242.243565	29.846823
395.636197	20272.993382	29.851840
396.376984	20302.646159	29.856858
396.064632	20338.756695	29.861876
396.598311	20370.055285	29.866893
397.030449	20405.113677	29.871911
397.228671	20449.859889	29.876928
398.379446	20482.494060	29.881946
398.191514	20526.322384	29.886964
398.629972	20558.359235	29.891981
399.194964	20599.549541	29.896999
399.499090	20636.009230	29.902016
400.075675	20658.041659	29.907034
400.233761	20709.956313	29.912052
400.754190	20740.592452	29.917069
401.152560	20781.804575	29.922087
401.623180	20818.295339	29.927104
401.952771	20843.643744	29.932122
402.307071	20890.796403	29.937140
403.094491	20922.813824	29.942157
403.416793	20955.217590	29.947175
403.676008	20993.949604	29.952192
404.096351	21026.630483	29.957210
404.508852	21066.883917	29.962228
404.728531	21107.238849	29.967245
405.405779	21136.142118	29.972263
405.470713	21180.701134	29.977280
406.215319	21226.514363	29.982298
406.633094	21258.945425	29.987316
406.833283	21298.495209	29.992333
407.120355	21333.831903	29.997351
407.460057	21371.662156	30.002368
408.035497	21413.040345	30.007386
408.350759	21456.446930	30.012404
408.984951	21490.409741	30.017421
409.178840	21539.030395	30.022439
409.498079	21586.955531	30.027456
410.162446	21627.740818	30.032474
410.452230	21662.650456	30.037492
410.929555	21705.951927	30.042509
410.894319	21753.622644	30.047527
411.423433	21798.140874	30.052544
412.344628	21838.485094	30.057562
412.914598	21876.521049	30.062580
412.850292	21918.732044	30.067597
413.770318	21951.757440	30.072615
413.924875	21994.990276	30.077632
414.075938	22029.942634	30.082650
414.430157	22065.763231	30.087668
414.873238	22119.290481	30.092685
415.808311	22155.565082	30.097703
416.518283	22192.287113	30.102720
416.990121	22218.541102	30.107738
417.516733	22240.851957	30.112756
418.122446	22270.592134	30.117773
418.736072	22300.162333	30.122791
418.816639	22347.556891	30.127808
419.442524	22362.071518	30.132826
419.742169	22390.689609	30.137844
419.636257	22425.354339	30.142861
420.069682	22452.811863	30.147879
419.935138	22484.225369	30.152896
420.422183	22530.252056	30.157914
420.662737	22578.618806	30.162932
421.405180	22613.765851	30.167949
421.923404	22645.295139	30.172967
422.017764	22687.125328	30.177984
422.556429	22719.466577	30.183002
422.954877	22769.110103	30.188020
422.930597	22810.878307	30.193037
423.450135	22841.862157	30.198055
423.633515	22905.798016	30.203072
424.012371	22936.103709	30.208090
424.180550	22987.460732	30.213108
425.058249	23040.321071	30.218125
425.430113	23074.198178	30.223143
425.906459	23134.066815	30.228160
426.661263	23175.276024	30.233178
427.676305	23194.935134	30.238196
428.025772	23240.079894	30.243213
428.657442	23263.290812	30.248231
429.162790	23305.263981	30.253248
429.992857	23325.089579	30.258266
430.404552	23354.053365	30.263284
430.651794	23389.596493	30.268301
430.749209	23408.121524	30.273319
431.128044	23445.033729	30.278336
431.671753	23485.271117	30.283354
432.218073	23517.243620	30.288372
431.946986	23561.964042	30.293389
432.464565	23603.467574	30.298407
432.828994	23653.589250	30.303424
432.979989	23685.321809	30.308442
433.326531	23738.909617	30.313460
433.460249	23792.187595	30.318477
434.166455	23835.216788	30.323495
434.250238	23888.933864	30.328512
434.947599	23939.459969	30.333530
435.352463	23992.848077	30.338548
435.773773	24042.881023	30.343565
436.194799	24098.455584	30.348583
436.752425	24148.459890	30.353600
437.022032	24200.442386	30.358618
437.535611	24248.990879	30.363636
437.575277	24305.670254	30.368653
438.827241	24351.052835	30.373671
439.123319	24401.265328	30.378688
439.499205	24451.461558	30.383706
439.973907	24510.532610	30.388724
440.524568	24550.667272	30.393741
441.194588	24596.185010	30.398759
441.634477	24649.077324	30.403776
442.466814	24679.299756	30.408794
443.136279	24717.364966	30.413812
443.782248	24765.161201	30.418829
444.162226	24796.556578	30.423847
444.528033	24832.814751	30.428864
445.080325	24860.119214	30.433882
445.727887	24887.625526	30.438900
445.610704	24937.110253	30.443917
446.086223	24969.098812	30.448935
446.379129	25013.598449	30.453952
446.956428	25053.654169	30.458970
447.252276	25094.497942	30.463988
447.436194	25141.217570	30.469005
447.890785	25177.291403	30.474023
448.193103	25221.591307	30.479040
448.628755	25265.121652	30.484058
449.002324	25319.023751	30.489076
449.410108	25358.461740	30.494093
449.952824	25407.648967	30.499111
450.426343	25469.202681	30.504128
451.107515	25505.075553	30.509146
451.512340	25545.012820	30.514164
451.449590	25582.138607	30.519181
452.028137	25613.944085	30.524199
452.532635	25675.370378	30.529216
452.540361	25714.806237	30.534234
453.207060	25757.608683	30.539252
453.533988	25809.520292	30.544269
454.194763	25851.560633	30.549287
454.781576	25902.164510	30.554304
454.781208	25950.352122	30.559322
455.629144	26001.767724	30.564340
456.320688	26060.934263	30.569357
456.477502	26108.966886	30.574375
456.915544	26149.710689	30.579392
457.284529	26197.490674	30.584410
458.027838	26249.000095	30.589428
458.222548	26305.584603	30.594445
458.231277	26354.844300	30.599463
458.974935	26405.032467	30.604480
460.030659	26460.802607	30.609498
460.574264	26500.394142	30.614516
460.795119	26558.902446	30.619533
461.156500	26606.079187	30.624551
461.802627	26651.514862	30.629568
461.967069	26706.049054	30.634586
462.484396	26750.484359	30.639604
462.603904	26810.962920	30.644621
462.666666	26862.536731	30.649639
463.427276	26920.458214	30.654656
464.067700	26982.216722	30.659674
465.063163	27031.103112	30.664692
465.482186	27090.637040	30.669709
465.890815	27142.759898	30.674727
466.490294	27196.605104	30.679744
466.620145	27262.663795	30.684762
467.301627	27305.363528	30.689780
467.872918	27358.157161	30.694797
468.397924	27412.712554	30.699815
468.937460	27457.556074	30.704832
469.031915	27516.706892	30.709850
469.611085	27569.392605	30.714868
469.538349	27632.823914	30.719885
470.399557	27683.583016	30.724903
471.315235	27726.579275	30.729920
471.860964	27783.141854	30.734938
472.211610	27841.513055	30.739956
472.685660	27892.785023	30.744973
473.261686	27932.204099	30.749991
473.579573	27990.533921	30.755008
473.792806	28043.051561	30.760026
474.488935	28090.284000	30.765044
474.587703	28146.262674	30.770061
474.974429	28203.972931	30.775079
475.788395	28258.940415	30.780096
475.773801	28322.777842	30.785114
476.285434	28368.243509	30.790132
476.590273	28435.170365	30.795149
477.224238	28491.622798	30.800167
477.916072	28559.924409	30.805184
478.274334	28623.234110	30.810202
478.944764	28678.283542	30.815220
479.382758	28745.877211	30.820237
480.067543	28785.895336	30.825255
480.512023	28837.755473	30.830272
480.770391	28896.508332	30.835290
481.480089	28959.334988	30.840308
481.773287	29015.640650	30.845325
482.248675	29072.758571	30.850343
482.642042	29113.728125	30.855360
482.833647	29187.213467	30.860378
483.601692	29233.541088	30.865396
484.082412	29283.229149	30.870413
484.235049	29337.319244	30.875431
484.784308	29401.865144	30.880448
485.263928	29464.567774	30.885466
486.074728	29517.706762	30.890484
486.390199	29580.219380	30.895501
486.667435	29641.874123	30.900519
487.436959	29702.125408	30.905536
487.620393	29755.571226	30.910554
488.384447	29807.822856	30.915572
488.481884	29880.373948	30.920589
489.378397	29941.545144	30.925607
489.612180	29997.472612	30.930624
490.210321	30067.546688	30.935642
490.928801	30112.660730	30.940660
491.403473	30183.689657	30.945677
491.873397	30236.672897	30.950695
492.507652	30296.617412	30.955712
492.317315	30374.622916	30.960730
493.151244	30437.509964	30.965748
493.668854	30499.891322	30.970765
494.286969	30568.004775	30.975783
495.102563	30616.669232	30.980800
495.431783	30688.737140	30.985818
496.161212	30733.914062	30.990836
496.505623	30812.047240	30.995853
497.009361	30866.386622	31.000871
497.578750	30934.853498	31.005888
497.577987	30992.918101	31.010906
498.510836	31046.729276	31.015924
498.870757	31109.678516	31.020941
499.359521	31182.403464	31.025959
499.834162	31238.503115	31.030976
500.240703	31294.730996	31.035994
500.839315	31355.688394	31.041012
501.257869	31431.587566	31.046029
501.898558	31490.790440	31.051047
502.595839	31552.129692	31.056064
502.780364	31620.729404	31.061082
503.442024	31682.680837	31.066100
503.888478	31744.598812	31.071117
504.283156	31809.071934	31.076135
505.489425	31871.608820	31.081152
505.609057	31936.598227	31.086170
506.505137	31979.564022	31.091188
506.945405	32043.358339	31.096205
507.426214	32107.404893	31.101223
507.801156	32160.094148	31.106240
508.305744	32224.386450	31.111258
509.046211	32288.564082	31.116276
509.488321	32341.589815	31.121293
510.605755	32391.783588	31.126311
510.982834	32433.416743	31.131328
511.458176	32494.581551	31.136346
511.966391	32545.088348	31.141364
512.574129	32586.696178	31.146381
512.827871	32640.722810	31.151399
513.272598	32691.398339	31.156416
513.503548	32752.317474	31.161434
513.791529	32801.286992	31.166452
514.587531	32871.960966	31.171469
514.562541	32929.029328	31.176487
515.252026	32991.403553	31.181504
515.466185	33048.845956	31.186522
515.928857	33115.647623	31.191540
516.574760	33173.596191	31.196557
516.784557	33237.013382	31.201575
517.228606	33295.125246	31.206592
517.584285	33376.079467	31.211610
518.311491	33437.088931	31.216628
518.800579	33510.858405	31.221645
519.175846	33571.567038	31.226663
519.689021	33642.243703	31.231680
519.685399	33715.193336	31.236698
519.977011	33789.362810	31.241716
520.559330	33872.888218	31.246733
521.236193	33951.232455	31.251751
521.992855	34028.361461	31.256768
522.185661	34104.271663	31.261786
522.824068	34178.893230	31.266804
523.933510	34270.105512	31.271821
524.229908	34344.225999	31.276839
524.908234	34422.297506	31.281856
525.776497	34483.769953	31.286874
526.315284	34556.424653	31.291892
527.170589	34622.999494	31.296909
527.671242	34690.479238	31.301927
528.376444	34746.229769	31.306944
528.673164	34820.835015	31.311962
529.091329	34888.338669	31.316980
529.647327	34964.337366	31.321997
530.210455	35038.646805	31.327015
530.902524	35103.925072	31.332032
531.216456	35167.003591	31.337050
531.732857	35242.445133	31.342068
532.338086	35308.748458	31.347085
533.068742	35375.665541	31.352103
533.697219	35439.993028	31.357120
534.023606	35516.650756	31.362138
534.263364	35577.701125	31.367156
535.277009	35649.902672	31.372173
535.513276	35719.282747	31.377191
536.128983	35782.679405	31.382208
536.711133	35855.691940	31.387226
536.908556	35937.264706	31.392244
537.947358	35991.193164	31.397261
538.168811	36067.204732	31.402279
539.040749	36131.693091	31.407296
539.743234	36205.703314	31.412314
540.647455	36255.492041	31.417332
541.278060	36318.241108	31.422349
542.194514	36372.522417	31.427367
542.463886	36418.131020	31.432384
543.171566	36487.650379	31.437402
543.247283	36539.007202	31.442420
543.626281	36598.633417	31.447437
544.296004	36667.496979	31.452455
544.846227	36729.800024	31.457472
545.579470	36803.435159	31.462490
545.751554	36857.576419	31.467508
546.562270	36926.029339	31.472525
546.627933	36990.866124	31.477543
546.951686	37065.166849	31.482560
547.326026	37135.062829	31.487578
547.931714	37206.520881	31.492596
548.706397	37278.923283	31.497613
549.066443	37355.939875	31.502631
549.513474	37416.393897	31.507648
549.991549	37484.954667	31.512666
550.318635	37574.195718	31.517684
551.040288	37657.601903	31.522701
551.536916	37729.225314	31.527719
552.032644	37805.889864	31.532736
552.457782	37874.757592	31.537754
552.684260	37952.461728	31.542772
553.557142	38019.001989	31.547789
553.630615	38105.576413	31.552807
554.709449	38180.213983	31.557824
555.501807	38256.736479	31.562842
556.179106	38326.031191	31.567860
556.830200	38384.368128	31.572877
557.378883	38465.376262	31.577895
557.639796	38529.119210	31.582912
558.496247	38603.656559	31.587930
558.735892	38676.131273	31.592948
559.574775	38744.529545	31.597965
560.354680	38805.595770	31.602983
560.909270	38874.796151	31.608000
561.571813	38949.701707	31.613018
561.794081	39027.256443	31.618036
562.620108	39089.584900	31.623053
563.002065	39178.370134	31.628071
563.683812	39240.656776	31.633088
564.377888	39314.636860	31.638106
564.634198	39382.177802	31.643124
565.270445	39455.552515	31.648141
565.946704	39537.197635	31.653159
566.158360	39610.861284	31.658176
566.788634	39686.103503	31.663194
567.051958	39765.242354	31.668212
567.796334	39853.664473	31.673229
568.278332	39934.273492	31.678247
568.874676	40024.015271	31.683264
568.971425	40098.517550	31.688282
569.718114	40169.862767	31.693300
570.559518	40256.752307	31.698317
570.723929	40361.410654	31.703335
571.569731	40437.330438	31.708352
572.554634	40515.891799	31.713370
573.312179	40600.388228	31.718388
574.034558	40669.277081	31.723405
574.423544	40744.582638	31.728423
575.198005	40824.244123	31.733440
576.243737	40890.440957	31.738458
576.903425	40976.170762	31.743476
577.334665	41032.064986	31.748493
577.642414	41110.902330	31.753511
578.360154	41176.621136	31.758528
579.161485	41249.808270	31.763546
579.256959	41322.421529	31.768564
579.994315	41387.683225	31.773581
580.751312	41472.906686	31.778599
581.007244	41552.575334	31.783616
581.794004	41618.928279	31.788634
581.877654	41694.272620	31.793652
582.569335	41772.010363	31.798669
583.049093	41852.890165	31.803687
583.658188	41945.944603	31.808704
584.277720	42007.521647	31.813722
584.827117	42089.363297	31.818740
585.594889	42160.535905	31.823757
586.174732	42245.972292	31.828775
586.229622	42333.245294	31.833792
587.060779	42416.459152	31.838810
587.344685	42502.040571	31.843828
588.117789	42591.850700	31.848845
588.327576	42670.000568	31.853863
589.407746	42760.410905	31.858880
589.986366	42825.981853	31.863898
590.725172	42913.106120	31.868916
591.378914	42987.000262	31.873933
591.885716	43063.719586	31.878951
592.375747	43129.723072	31.883968
592.948934	43206.419331	31.888986
593.200164	43289.572365	31.894004
593.799186	43364.061187	31.899021
594.686030	43448.173398	31.904039
595.085219	43533.525706	31.909056
596.025343	43608.385104	31.914074
596.251479	43699.191235	31.919092
596.547502	43769.482169	31.924109
597.340667	43864.621593	31.929127
598.090627	43942.576579	31.934144
598.767777	44026.776730	31.939162
598.890814	44112.490116	31.944180
599.549320	44197.287727	31.949197
600.321226	44283.895064	31.954215
600.666775	44390.431001	31.959232
601.344984	44473.685737	31.964250
601.731463	44566.973338	31.969268
602.643608	44663.663186	31.974285
603.545540	44739.063909	31.979303
603.788504	44835.572106	31.984320
604.415567	44917.681635	31.989338
605.034567	45013.610462	31.994356
605.975585	45100.638703	31.999373
606.395501	45189.329525	32.004391
606.846809	45293.772143	32.009408
607.894699	45381.011284	32.014426
608.320605	45473.106392	32.019444
608.909810	45557.766917	32.024461
609.388671	45653.090731	32.029479
609.873892	45752.531625	32.034496
610.613339	45852.587636	32.039514
610.828084	45935.591069	32.044532
611.848465	46031.616310	32.049549
612.929920	46121.455292	32.054567
613.237731	46221.584926	32.059584
613.993766	46307.086339	32.064602
614.832496	46409.598213	32.069620
615.858368	46489.829453	32.074637
616.505852	46566.018661	32.079655
616.943543	46657.407058	32.084672
617.300628	46744.132462	32.089690
617.822433	46825.279340	32.094708
618.585322	46899.789675	32.099725
619.521735	46988.327375	32.104743
619.770598	47080.740747	32.109760
620.503081	47167.598385	32.114778
620.766184	47276.014822	32.119796
621.688030	47365.538824	32.124813
622.142671	47447.258469	32.129831
622.357564	47536.464855	32.134848
623.174920	47632.418218	32.139866
623.874688	47724.099813	32.144884
624.272059	47813.773008	32.149901
624.991019	47919.714132	32.154919
625.144609	48032.255383	32.159936
626.175283	48122.267004	32.164954
626.950493	48220.229400	32.169972
627.609023	48307.900357	32.174989
628.195975	48395.612023	32.180007
628.397877	48491.725581	32.185024
629.396710	48587.479909	32.190042
629.882878	48700.143562	32.195060
630.278943	48795.019969	32.200077
631.168128	48901.658337	32.205095
631.729868	48995.292305	32.210112
632.536992	49075.327564	32.215130
633.105120	49170.483608	32.220148
633.157201	49263.022308	32.225165
634.230431	49358.360712	32.230183
634.784292	49465.228434	32.235200
635.916497	49528.475646	32.240218
636.634235	49622.124665	32.245236
637.580300	49699.729634	32.250253
638.335385	49781.579901	32.255271
638.437840	49879.037107	32.260288
638.875581	49968.533637	32.265306
639.274082	50050.643232	32.270324
640.431065	50149.638577	32.275341
641.054870	50236.922978	32.280359
642.068023	50329.979975	32.285376
642.662815	50412.298559	32.290394
643.525524	50495.198392	32.295412
643.864987	50583.302242	32.300429
644.552727	50668.089070	32.305447
644.926865	50755.151948	32.310464
645.535333	50851.790941	32.315482
645.975058	50950.789457	32.320500
646.702076	51054.920855	32.325517
647.383438	51138.036749	32.330535
647.545531	51241.580689	32.335552
648.378693	51329.151115	32.340570
649.280550	51427.310943	32.345588
649.765477	51533.323434	32.350605
650.270323	51626.110966	32.355623
650.737026	51745.987926	32.360640
651.752838	51840.713211	32.365658
652.243495	51952.450622	32.370676
652.842754	52061.169831	32.375693
653.787794	52156.634915	32.380711
654.054185	52271.210053	32.385728
655.200969	52358.322398	32.390746
655.819010	52468.190559	32.395764
656.621955	52568.988062	32.400781
657.703275	52657.439322	32.405799
658.193507	52747.783353	32.410816
659.050028	52838.755621	32.415834
660.007317	52940.508666	32.420852
660.524788	53033.414513	32.425869
661.221916	53126.486825	32.430887
661.740927	53217.226269	32.435904
662.433301	53309.194611	32.440922
662.950886	53388.506006	32.445940
663.720067	53487.260520	32.450957
664.856296	53575.921626	32.455975
665.617390	53655.755973	32.460992
666.325857	53740.161006	32.466010
667.286504	53836.737356	32.471028
667.367329	53921.108374	32.476045
667.962250	53998.589782	32.481063
668.595811	54086.944929	32.486080
669.505907	54183.683012	32.491098
670.025665	54262.138299	32.496116
670.521124	54355.982831	32.501133
671.365776	54443.451569	32.506151
671.527930	54545.515538	32.511168
672.149718	54638.936070	32.516186
672.727599	54733.628006	32.521204
673.001925	54839.440609	32.526221
673.847630	54926.936588	32.531239
674.404569	55051.450159	32.536256
675.103771	55144.038826	32.541274
676.005703	55237.851653	32.546292
676.293576	55342.344124	32.551309
677.265912	55434.743477	32.556327
677.835212	55528.871969	32.561344
678.792317	55620.851372	32.566362
679.488124	55716.217159	32.571380
679.814458	55810.273589	32.576397
681.040157	55906.556989	32.581415
681.105246	56006.470952	32.586432
681.913550	56102.717182	32.591450
682.402953	56192.363104	32.596468
682.939936	56291.978995	32.601485
683.779030	56392.297174	32.606503
684.491888	56508.250863	32.611520
684.873562	56614.453192	32.616538
685.586502	56720.215630	32.621556
685.983416	56835.484353	32.626573
686.783537	56939.211389	32.631591
687.400659	57050.198386	32.636608
688.165533	57160.952937	32.641626
689.045671	57267.271872	32.646644
689.521249	57384.780322	32.651661
690.275016	57499.582879	32.656679
691.025939	57618.380344	32.661696
691.712187	57742.876629	32.666714
692.598005	57843.661966	32.671732
694.147175	57933.582108	32.676749
695.530869	58017.495103	32.681767
696.208160	58127.277392	32.686784
696.881268	58212.528825	32.691802
697.536379	58293.378927	32.696820
697.945072	58396.451751	32.701837
698.625831	58487.561272	32.706855
699.330760	58590.364724	32.711872
699.515033	58690.651461	32.716890
700.375480	58791.553198	32.721908
701.026651	58898.873052	32.726925
701.842378	58997.634555	32.731943
702.584313	59100.706213	32.736960
703.012334	59203.792593	32.741978
703.974259	59318.469857	32.746996
704.304523	59412.100144	32.752013
704.960727	59526.380633	32.757031
705.639658	59642.225330	32.762048
706.002221	59749.957850	32.767066
707.016417	59861.456903	32.772084
707.391955	59983.452693	32.777101
708.347529	60094.356038	32.782119
708.734880	60215.738218	32.787136
709.521151	60322.878868	32.792154
710.294631	60433.890140	32.797172
710.478063	60556.275188	32.802189
711.780708	60678.740614	32.807207
712.284815	60791.700946	32.812224
712.616160	60920.042591	32.817242
713.476013	61036.200173	32.822260
714.298955	61168.614232	32.827277
714.941924	61287.179390	32.832295
715.633451	61405.610766	32.837312
715.945633	61533.883604	32.842330
716.783201	61653.758526	32.847348
717.357523	61787.235470	32.852365
718.521581	61911.140786	32.857383
719.271852	62034.831117	32.862400
720.153553	62163.544281	32.867418
721.028666	62276.008769	32.872436
721.702457	62405.838812	32.877453
722.805221	62527.627933	32.882471
723.309090	62644.530061	32.887488
723.930242	62747.893049	32.892506
725.106275	62862.213369	32.897524
725.482493	62971.736774	32.902541
726.236561	63073.568627	32.907559
726.975070	63182.660071	32.912576
727.682222	63303.748299	32.917594
728.720535	63398.613037	32.922612
729.457321	63514.014942	32.927629
730.079610	63612.015459	32.932647
730.680429	63730.228761	32.937664
731.109905	63841.966667	32.942682
731.960035	63958.142384	32.947700
732.665851	64071.049328	32.952717
733.144195	64175.637887	32.957735
734.213982	64298.877872	32.962752
734.512604	64425.685438	32.967770
735.065049	64537.217034	32.972788
736.328661	64669.226446	32.977805
737.088968	64786.332000	32.982823
737.881390	64899.108961	32.987840
738.721924	65026.683634	32.992858
739.588050	65140.770875	32.997876
739.499280	65267.458229	33.002893
740.146167	65388.581269	33.007911
741.228435	65517.471652	33.012928
741.502559	65643.658524	33.017946
742.457773	65774.487074	33.022964
742.733389	65913.299934	33.027981
743.856369	66047.263253	33.032999
744.798336	66184.905221	33.038016
745.395770	66318.906946	33.043034
746.520488	66441.625753	33.048052
747.070536	66570.143143	33.053069
748.086958	66709.103815	33.058087
748.907178	66843.704112	33.063104
749.594951	66966.315179	33.068122
750.693391	67078.009926	33.073140
751.242591	67212.158118	33.078157
751.864422	67332.120607	33.083175
753.323699	67466.821113	33.088192
754.094935	67590.389267	33.093210
755.167146	67706.346629	33.098228
755.867699	67825.002767	33.103245
756.497004	67938.632415	33.108263
757.484259	68060.751234	33.113280
757.963905	68184.782227	33.118298
758.585751	68294.204232	33.123316
759.190647	68423.710120	33.128333
759.607604	68550.712626	33.133351
760.489495	68673.111691	33.138368
760.916118	68809.800450	33.143386
762.025515	68934.306647	33.148404
762.688100	69052.767306	33.153421
763.762326	69184.653155	33.158439
764.548656	69315.683445	33.163456
764.924348	69436.097036	33.168474
765.984053	69565.041188	33.173492
766.510632	69695.788140	33.178509
766.911315	69827.638023	33.183527
768.029402	69958.092376	33.188544
768.676157	70097.699379	33.193562
769.727288	70223.032126	33.198580
770.409988	70347.560494	33.203597
771.030597	70477.025656	33.208615
771.998332	70608.065369	33.213632
772.745915	70744.896599	33.218650
773.691262	70865.539829	33.223668
774.350398	71004.353941	33.228685
774.642052	71129.862319	33.233703
775.880112	71246.203461	33.238720
776.331547	71383.467317	33.243738
776.844097	71501.599662	33.248756
777.205664	71622.021539	33.253773
778.182220	71756.563690	33.258791
779.021463	71886.133827	33.263808
779.538477	72029.208615	33.268826
780.576131	72149.470612	33.273844
781.499798	72283.512605	33.278861
782.691297	72431.113372	33.283879
783.785602	72541.762356	33.288896
784.194137	72680.363235	33.293914
784.587261	72809.823236	33.298932
785.827403	72941.862689	33.303949
786.281360	73081.280691	33.308967
787.378293	73213.117902	33.313984
787.893448	73346.254047	33.319002
788.533268	73471.699223	33.324020
789.427782	73612.856179	33.329037
790.039477	73760.277629	33.334055
791.022115	73893.579832	33.339072
791.529359	74035.202225	33.344090
792.426463	74170.221530	33.349108
793.331945	74310.483126	33.354125
793.890809	74457.943343	33.359143
794.931054	74591.240234	33.364160
795.732002	74747.927443	33.369178
796.952438	74879.551824	33.374196
797.811763	75028.483872	33.379213
798.325450	75177.189696	33.384231
799.102061	75303.387924	33.389248
799.694568	75464.421883	33.394266
800.653138	75599.072940	33.399284
801.326160	75743.936035	33.404301
801.817946	75896.552695	33.409319
802.768884	76049.353510	33.414336
803.288657	76204.877060	33.419354
804.307149	76361.311929	33.424372
805.223745	76512.862989	33.429389
805.744972	76663.797615	33.434407
807.037677	76796.990030	33.439424
808.225354	76957.101153	33.444442
809.312037	77098.956965	33.449460
810.113425	77237.331607	33.454477
810.682414	77379.003153	33.459495
811.588748	77523.592459	33.464512
812.100929	77672.580933	33.469530
813.121434	77820.296868	33.474548
813.924918	77958.251839	33.479565
814.536424	78112.211131	33.484583
815.367993	78252.130449	33.489600
815.912583	78404.546801	33.494618
816.890546	78558.808888	33.499636
817.938009	78702.073005	33.504653
818.834422	78858.722773	33.509671
819.713668	79003.288179	33.514688
820.423553	79150.235780	33.519706
821.108663	79297.422504	33.524724
822.142545	79437.935549	33.529741
822.660865	79589.213003	33.534759
823.963804	79723.294105	33.539776
824.557728	79883.948537	33.544794
825.316168	80033.253386	33.549812
826.781611	80166.911617	33.554829
827.476449	80302.608998	33.559847
828.538568	80431.148412	33.564864
829.726592	80573.388920	33.569882
830.325215	80706.789346	33.574900
831.195853	80836.805196	33.579917
831.819371	80972.202112	33.584935
832.503614	81079.640494	33.589952
833.373737	81212.378852	33.594970
834.096011	81346.743077	33.599988
834.891642	81473.719416	33.605005
835.667843	81618.293316	33.610023
836.248592	81738.626149	33.615040
836.705184	81877.358529	33.620058
837.618471	82017.426754	33.625076
838.641439	82166.328434	33.630093
839.019569	82318.918947	33.635111
840.061371	82458.993848	33.640128
840.564556	82604.327870	33.645146
841.214032	82761.943931	33.650164
842.947502	82898.205601	33.655181
843.446632	83053.862027	33.660199
844.483303	83197.757325	33.665216
845.264755	83346.143656	33.670234
846.005669	83492.070185	33.675252
846.937500	83646.406069	33.680269
847.719011	83806.253418	33.685287
848.757953	83946.913602	33.690304
849.677646	84105.095059	33.695322
850.207597	84257.647898	33.700340
851.415829	84401.724688	33.705357
852.152220	84562.559125	33.710375
852.935134	84716.003086	33.715392
854.243694	84860.546942	33.720410
854.855073	85014.173195	33.725428
855.886874	85161.567851	33.730445
856.572664	85317.278103	33.735463
857.801800	85457.624812	33.740480
858.632854	85614.882141	33.745498
859.397908	85759.249699	33.750516
860.538244	85903.024349	33.755533
860.993282	86049.843293	33.760551
861.902829	86203.339294	33.765568
862.739982	86359.879266	33.770586
863.511181	86508.743065	33.775604
865.294055	86643.563158	33.780621
865.800925	86792.586527	33.785639
866.811363	86939.477048	33.790656
868.147739	87076.012635	33.795674
868.642366	87234.152946	33.800692
869.682600	87365.234087	33.805709
870.767421	87509.806122	33.810727
871.345386	87643.705545	33.815744
872.490447	87789.110915	33.820762
873.303645	87928.389719	33.825780
874.008199	88069.573153	33.830797
874.645447	88215.850112	33.835815
875.619754	88357.199318	33.840832
876.485811	88505.142370	33.845850
877.185248	88654.423951	33.850868
878.518546	88782.471022	33.855885
880.047526	88917.706951	33.860903
880.723876	89053.306651	33.865920
881.607003	89179.595341	33.870938
882.517039	89323.580920	33.875956
883.174748	89452.528447	33.880973
883.904045	89611.873368	33.885991
884.518669	89743.487598	33.891008
885.613364	89879.351640	33.896026
886.226371	90026.080400	33.901044
886.816818	90164.390329	33.906061
887.902141	90305.511145	33.911079
888.934789	90461.267284	33.916096
889.718694	90582.124450	33.921114
890.556523	90723.314110	33.926132
891.644182	90850.526984	33.931149
892.507093	90982.239699	33.936167
893.440355	91121.409594	33.941184
894.226194	91238.573637	33.946202
895.226972	91380.537550	33.951220
895.923243	91516.818729	33.956237
896.565373	91652.166629	33.961255
897.301987	91789.480614	33.966272
898.434481	91939.976570	33.971290
899.008738	92082.553361	33.976308
900.065255	92219.563521	33.981325
900.649616	92377.596318	33.986343
901.374186	92530.467481	33.991360
902.409645	92671.698995	33.996378
903.778311	92826.268980	34.001396
904.433108	92971.951665	34.006413
905.568485	93130.176387	34.011431
905.973392	93276.940393	34.016448
906.727922	93436.040474	34.021466
907.631096	93605.079668	34.026484
908.529171	93757.986682	34.031501
909.529140	93917.985941	34.036519
910.469813	94085.180289	34.041536
911.293698	94251.205166	34.046554
911.923808	94423.776669	34.051572
912.768422	94592.528543	34.056589
913.634053	94758.277725	34.061607
914.212316	94941.660216	34.066624
915.085660	95113.518872	34.071642
916.089600	95303.777373	34.076660
917.060937	95461.905055	34.081677
917.791558	95648.350228	34.086695
918.866373	95828.010735	34.091712
920.049510	96013.528982	34.096730
920.764473	96201.936934	34.101748
921.632619	96375.166186	34.106765
922.765009	96561.994647	34.111783
923.585815	96747.375915	34.116800
924.608598	96925.356426	34.121818
925.190582	97114.869504	34.126836
926.515723	97289.732149	34.131853
927.601048	97478.721309	34.136871
928.921725	97657.176686	34.141888
929.963550	97831.836901	34.146906
930.470975	98011.955443	34.151924
931.596199	98172.739961	34.156941
933.061504	98352.727299	34.161959
933.739952	98529.117644	34.166976
934.784941	98694.711237	34.171994
935.669844	98874.887245	34.177012
936.452920	99043.692042	34.182029
937.366254	99218.376835	34.187047
938.205606	99408.795087	34.192064
939.348348	99578.214841	34.197082
940.253092	99761.698675	34.202100
941.112072	99932.978584	34.207117
941.922020	100116.392065	34.212135
942.558308	100301.931330	34.217152
944.123097	100473.794177	34.222170
944.902364	100658.216983	34.227188
945.805071	100835.548457	34.232205
947.220270	101009.155530	34.237223
947.796569	101188.689969	34.242240
949.102489	101359.981231	34.247258
949.814186	101544.598895	34.252276
950.662324	101705.958211	34.257293
951.560947	101880.081103	34.262311
952.267053	102048.994471	34.267328
953.508345	102213.957771	34.272346
954.176531	102377.370965	34.277364
955.213574	102558.756999	34.282381
955.952597	102724.775669	34.287399
956.629616	102905.267757	34.292416
957.623726	103067.928370	34.297434
958.388211	103262.528662	34.302452
959.373566	103449.849902	34.307469
960.183817	103639.056845	34.312487
960.953611	103830.120852	34.317504
961.924248	104020.861646	34.322522
962.962634	104208.793744	34.327540
963.767849	104401.337779	34.332557
964.423927	104588.462184	34.337575
966.068597	104781.464940	34.342592
967.560197	104963.324154	34.347610
969.879757	105133.129569	34.352628
971.019248	105285.261640	34.357645
972.647876	105439.377820	34.362663
973.462409	105610.677232	34.367680
974.436123	105761.307074	34.372698
975.205512	105923.459071	34.377716
975.822454	106087.752468	34.382733
977.107706	106251.315377	34.387751
977.538336	106415.540394	34.392768
978.467829	106589.144831	34.397786
979.007201	106749.034896	34.402804
979.988685	106936.349877	34.407821
981.201952	107108.555371	34.412839
981.907957	107291.156201	34.417856
982.936952	107469.018260	34.422874
983.811682	107645.678488	34.427892
984.661705	107842.635183	34.432909
985.382668	108019.589377	34.437927
986.273951	108208.055510	34.442944
986.999370	108399.907091	34.447962
988.013338	108591.940152	34.452980
989.179982	108787.128566	34.457997
990.453922	108975.865897	34.463015
991.370683	109174.822585	34.468032
992.640010	109357.115940	34.473050
993.707166	109547.956271	34.478068
994.686142	109736.823847	34.483085
995.896958	109927.034982	34.488103
996.942326	110129.448117	34.493120
997.936178	110306.549307	34.498138
998.725810	110485.509639	34.503156
999.710996	110680.247726	34.508173
1000.534248	110873.519292	34.513191
1001.558178	111075.930320	34.518208
1002.576147	111259.975563	34.523226
1003.244296	111445.448212	34.528244
1004.410175	111649.360050	34.533261
1005.787792	111832.766720	34.538279
1007.374665	112022.435941	34.543296
1008.570335	112196.006756	34.548314
1009.824391	112367.364692	34.553332
1010.602482	112546.441683	34.558349
1012.060499	112719.921578	34.563367
1013.327082	112885.807878	34.568384
1014.632168	113048.914360	34.573402
1015.623005	113215.621166	34.578420
1016.343728	113378.598506	34.583437
1017.595282	113537.016630	34.588455
1018.222607	113712.160801	34.593472
1018.792715	113879.346786	34.598490
1020.022866	114042.813574	34.603508
1020.361042	114217.818849	34.608525
1021.417798	114381.772472	34.613543
1022.105397	114561.802255	34.618560
1022.997115	114721.832434	34.623578
1024.253252	114910.663991	34.628596
1024.626140	115097.375525	34.633613
1025.464501	115275.915189	34.638631
1026.222921	115475.475563	34.643648
1027.334997	115652.983956	34.648666
1028.367903	115849.625386	34.653684
1029.401035	116048.662758	34.658701
1030.457371	116244.454147	34.663719
1031.200771	116456.073096	34.668736
1032.394090	116644.166415	34.673754
1033.520107	116842.307006	34.678772
1035.107542	117048.494122	34.683789
1036.120377	117228.981000	34.688807
1036.873955	117434.282941	34.693824
1038.043216	117635.412092	34.698842
1039.140668	117830.409265	34.703860
1039.461925	118042.756178	34.708877
1041.244452	118237.135601	34.713895
1042.295282	118451.265102	34.718912
1042.980681	118659.881543	34.723930
1044.117501	118868.475270	34.728948
1044.497601	119070.087472	34.733965
1045.714000	119290.556675	34.738983
1046.474626	119502.980768	34.744000
1047.606694	119724.430279	34.749018
1049.018365	119946.886824	34.754036
1049.635358	120160.999521	34.759053
1050.854194	120386.101779	34.764071
1052.489082	120609.983588	34.769088
1054.350802	120782.659865	34.774106
1056.098608	120989.836810	34.779124
1057.128074	121196.982331	34.784141
1058.763648	121378.962999	34.789159
1059.849821	121581.108937	34.794176
1060.690496	121757.508594	34.799194
1062.011087	121949.074697	34.804212
1063.127550	122135.670233	34.809229
1064.399928	122312.609849	34.814247
1065.472913	122491.750639	34.819264
1066.100806	122675.997461	34.824282
1067.191329	122863.539652	34.829300
1067.741324	123058.713123	34.834317
1069.150515	123253.314430	34.839335
1069.758609	123447.061410	34.844352
1070.472723	123645.658567	34.849370
1071.602966	123847.153550	34.854388
1072.339768	124052.200342	34.859405
1073.468479	124258.526896	34.864423
1074.242641	124472.327722	34.869440
1075.289784	124688.011166	34.874458
1076.569922	124905.393793	34.879476
1077.765158	125115.529953	34.884493
1078.728767	125324.400582	34.889511
1079.678007	125532.844112	34.894528
1080.211804	125755.768449	34.899546
1081.854312	125968.206344	34.904564
1082.388659	126191.995616	34.909581
1083.629397	126410.079924	34.914599
1084.983588	126624.344619	34.919616
1085.569401	126853.567521	34.924634
1086.904215	127069.397503	34.929652
1087.896860	127299.240653	34.934669
1088.974508	127518.817469	34.939687
1090.187613	127734.114596	34.944704
1091.303172	127924.180794	34.949722
1093.276523	128122.268594	34.954740
1094.209348	128313.875829	34.959757
1095.562623	128522.221856	34.964775
1096.424342	128718.786723	34.969792
1097.171026	128925.347454	34.974810
1098.620304	129123.477865	34.979828
1099.504888	129334.023868	34.984845
1100.237028	129532.174434	34.989863
1101.427385	129744.713241	34.994880
1102.458365	129967.395231	34.999898
1103.831841	130173.239065	35.004916
1104.733016	130380.430196	35.009933
1106.428028	130573.319137	35.014951
1107.719897	130781.373429	35.019968
1108.665243	130990.323205	35.024986
1109.998748	131183.199773	35.030004
1110.407802	131414.082595	35.035021
1111.475496	131615.803304	35.040039
1112.900196	131836.392174	35.045056
1113.578628	132048.422862	35.050074
1114.583325	132271.125346	35.055092
1115.583575	132495.123148	35.060109
1116.784059	132723.551567	35.065127
1118.050566	132943.388316	35.070144
1118.814043	133172.729096	35.075162
1120.246194	133396.496702	35.080180
1121.315438	133620.123223	35.085197
1122.427253	133857.537191	35.090215
1123.706332	134078.051453	35.095232
1124.502108	134314.646440	35.100250
1125.441367	134546.148283	35.105268
1126.756143	134789.214940	35.110285
1128.110000	135016.797303	35.115303
1128.825804	135263.757508	35.120320
1129.763159	135506.854055	35.125338
1131.439530	135738.051846	35.130356
1132.756297	135974.978060	35.135373
1133.690637	136211.132647	35.140391
1134.978203	136445.252492	35.145408
1135.866210	136691.155162	35.150426
1137.316184	136933.657320	35.155444
1138.259591	137174.089909	35.160461
1139.326057	137405.425843	35.165479
1140.940030	137643.100707	35.170496
1141.983275	137888.314452	35.175514
1143.527270	138109.978095	35.180532
1145.064028	138344.957429	35.185549
1145.802814	138580.501867	35.190567
1147.310525	138802.176077	35.195584
1148.052243	139044.367184	35.200602
1149.404161	139259.793957	35.205620
1150.470358	139499.208401	35.210637
1151.538094	139734.858430	35.215655
1152.542072	139974.311888	35.220672
1153.679699	140214.391518	35.225690
1155.285375	140430.468291	35.230708
1156.398282	140668.006545	35.235725
1157.866020	140888.483661	35.240743
1159.796775	141097.904409	35.245760
1161.576630	141300.466126	35.250778
1162.894471	141503.536801	35.255796
1163.978659	141722.345669	35.260813
1164.831706	141921.869322	35.265831
1166.101528	142118.801567	35.270848
1166.855250	142346.735720	35.275866
1167.924302	142543.678308	35.280884
1168.786789	142754.288024	35.285901
1169.472263	142954.403323	35.290919
1170.396069	143166.146609	35.295936
1171.319836	143365.362421	35.300954
1172.790267	143577.816405	35.305972
1173.767407	143790.936828	35.310989
1174.472785	144005.701440	35.316007
1175.690226	144228.295500	35.321024
1176.465508	144466.169199	35.326042
1178.192256	144675.049159	35.331060
1179.844826	144893.973691	35.336077
1180.849916	145113.843953	35.341095
1182.054408	145338.247876	35.346112
1182.791699	145557.518521	35.351130
1184.273318	145798.289480	35.356148
1185.369146	146017.604910	35.361165
1186.558735	146262.561703	35.366183
1187.225815	146496.383226	35.371200
1188.057499	146743.660045	35.376218
1189.241789	146978.629047	35.381236
1190.410589	147243.101143	35.386253
1190.899496	147494.726538	35.391271
1192.137458	147743.654871	35.396288
1192.809687	148014.974675	35.401306
1194.289375	148298.629594	35.406324
1195.014531	148559.823875	35.411341
1196.150938	148852.430606	35.416359
1197.822089	149116.617249	35.421376
1198.679594	149402.628727	35.426394
1200.183890	149669.878229	35.431412
1201.663287	149942.219749	35.436429
1203.117616	150227.770744	35.441447
1204.872575	150482.174329	35.446464
1206.224860	150755.316532	35.451482
1207.805180	151010.615140	35.456500
1209.035904	151274.027592	35.461517
1210.097459	151541.959989	35.466535
1212.060132	151794.980810	35.471552
1213.137594	152049.038023	35.476570
1214.175792	152301.530624	35.481588
1215.449480	152555.545976	35.486605
1216.738279	152829.297095	35.491623
1217.902474	153061.859641	35.496640
1219.385894	153324.775016	35.501658
1220.614624	153578.284525	35.506676
1222.589422	153812.746653	35.511693
1223.500576	154055.758454	35.516711
1225.234052	154297.341541	35.521728
1226.244210	154541.735270	35.526746
1227.760984	154782.976769	35.531764
1228.825526	155021.643622	35.536781
1230.015584	155270.870383	35.541799
1231.273448	155492.256458	35.546816
1232.490582	155749.206956	35.551834
1233.639457	155978.453253	35.556852
1234.842079	156212.157183	35.561869
1235.897453	156475.634091	35.566887
1237.122371	156709.134281	35.571904
1238.083771	156965.576911	35.576922
1239.321641	157220.415000	35.581940
1240.056130	157468.817760	35.586957
1241.235556	157735.263528	35.591975
1242.624784	157997.832447	35.596992
1243.153970	158270.948189	35.602010
1244.550354	158517.408159	35.607028
1246.041672	158789.568592	35.612045
1247.355552	159051.674761	35.617063
1248.915924	159299.520435	35.622080
1250.070087	159544.238030	35.627098
1251.367066	159789.707268	35.632116
1252.720803	160027.861145	35.637133
1253.850039	160270.582733	35.642151
1254.887196	160515.490434	35.647168
1257.270007	160728.941736	35.652186
1259.727873	160939.983893	35.657204
1260.968922	161158.828352	35.662221
1262.167138	161384.709603	35.667239
1263.567147	161592.720739	35.672256
1264.239974	161820.607214	35.677274
1265.193775	162032.741702	35.682292
1266.247184	162269.207395	35.687309
1267.164298	162493.682211	35.692327
1268.279588	162738.602651	35.697344
1269.160876	162977.803248	35.702362
1270.290610	163237.631839	35.707380
1271.127616	163485.584289	35.712397
1272.112185	163752.646605	35.717415
1273.712642	164020.521951	35.722432
1274.925667	164269.571151	35.727450
1275.947580	164550.741021	35.732468
1277.417331	164790.006387	35.737485
1278.357118	165072.005291	35.742503
1280.402592	165330.616162	35.747520
1281.562955	165608.483714	35.752538
1282.714005	165874.224632	35.757556
1283.950094	166142.478029	35.762573
1284.926405	166426.611248	35.767591
1286.161423	166705.589939	35.772608
1287.400287	166974.583869	35.777626
1288.291302	167276.475275	35.782644
1289.896402	167561.437756	35.787661
1292.021717	167827.625196	35.792679
1294.800230	168066.031497	35.797696
1296.592623	168310.363384	35.802714
1297.783284	168571.114437	35.807732
1299.673774	168797.985338	35.812749
1300.847740	169046.814193	35.817767
1302.272053	169288.344673	35.822784
1303.376794	169532.733762	35.827802
1304.396010	169774.473585	35.832820
1305.470662	170014.213256	35.837837
1306.551004	170272.403716	35.842855
1307.642469	170528.208147	35.847872
1308.926197	170776.165312	35.852890
1309.731584	171039.151573	35.857908
1311.328276	171300.599527	35.862925
1312.042256	171560.697944	35.867943
1313.224625	171836.544424	35.872960
1314.701399	172100.998872	35.877978
1315.371344	172384.725195	35.882996
1316.976610	172654.960795	35.888013
1317.984420	172945.537876	35.893031
1319.206855	173232.705529	35.898048
1320.538334	173513.270541	35.903066
1322.243138	173790.577304	35.908084
1324.194104	174043.301448	35.913101
1326.071829	174316.851575	35.918119
1327.984678	174576.729626	35.923136
1329.202319	174831.140464	35.928154
1330.481616	175102.332284	35.933172
1332.014857	175347.594213	35.938189
1333.049113	175603.651235	35.943207
1334.151963	175858.746399	35.948224
1335.543114	176120.267497	35.953242
1336.565558	176387.194079	35.958260
1337.875735	176639.327257	35.963277
1338.879452	176904.939854	35.968295
1340.051295	177154.598417	35.973312
1341.352499	177409.694057	35.978330
1342.436658	177675.221264	35.983348
1343.478443	177927.862351	35.988365
1344.905430	178194.338071	35.993383
1347.179239	178431.103304	35.998400
1349.112709	178672.444319	36.003418
1350.814625	178912.466865	36.008436
1352.295746	179151.486430	36.013453
1353.545987	179393.045694	36.018471
1355.038900	179623.638120	36.023488
1356.350744	179864.745169	36.028506
1357.699001	180090.540727	36.033524
1359.507048	180330.070003	36.038541
1361.035035	180568.415690	36.043559
1362.019060	180813.274925	36.048576
1363.406445	181043.561170	36.053594
1364.371408	181287.448481	36.058612
1365.887452	181526.054357	36.063629
1367.113077	181766.854494	36.068647
1368.107148	182021.541627	36.073664
1369.811681	182262.670761	36.078682
1370.869765	182517.032338	36.083700
1372.500112	182771.807937	36.088717
1373.756298	183025.593296	36.093735
1374.925807	183278.581888	36.098752
1376.746971	183526.031068	36.103770
1377.406623	183797.016238	36.108788
1378.572955	184058.399011	36.113805
1379.820610	184337.565180	36.118823
1380.766570	184618.052110	36.123840
1381.963219	184894.919429	36.128858
1382.777011	185200.957196	36.133876
1384.085019	185483.533644	36.138893
1385.498489	185784.842136	36.143911
1386.414857	186096.973330	36.148928
1387.320350	186405.185770	36.153946
1388.693427	186725.330482	36.158964
1390.629735	187040.725042	36.163981
1391.772071	187351.492866	36.168999
1393.072805	187667.072449	36.174016
1395.047182	187990.031441	36.179034
1395.952787	188323.997391	36.184052
1397.725819	188643.172553	36.189069
1399.357049	188962.436451	36.194087
1400.737237	189281.629476	36.199104
1402.214462	189588.837511	36.204122
1403.037407	189921.861544	36.209140
1404.587708	190238.340355	36.214157
1406.074633	190571.207154	36.219175
1407.322304	190895.724424	36.224192
1408.855344	191222.722345	36.229210
1409.739554	191559.566399	36.234228
1411.222869	191893.126613	36.239245
1412.656598	192224.145228	36.244263
1414.068138	192568.879729	36.249280
1415.712471	192904.741907	36.254298
1416.791552	193251.655394	36.259316
1418.477799	193582.436301	36.264333
1419.888211	193922.341697	36.269351
1421.399587	194260.962671	36.274368
1422.817147	194594.103976	36.279386
1424.487321	194931.991272	36.284404
1425.978101	195270.354441	36.289421
1427.581481	195598.569759	36.294439
1428.876805	195931.789072	36.299456
1430.863072	196243.998622	36.304474
1432.480431	196565.703690	36.309492
1433.839899	196861.833194	36.314509
1435.429082	197163.880245	36.319527
1436.595145	197475.000159	36.324544
1437.949772	197770.169648	36.329562
1439.454991	198085.108411	36.334580
1441.340684	198393.536007	36.339597
1442.721551	198691.650663	36.344615
1443.814221	199006.458990	36.349632
1445.258416	199314.379955	36.354650
1446.556451	199635.670253	36.359668
1448.275257	199958.568189	36.364685
1449.357098	200267.150214	36.369703
1450.428068	200593.903931	36.374720
1452.060523	200914.738408	36.379738
1453.493504	201240.787591	36.384756
1454.731001	201570.336847	36.389773
1456.201104	201901.867821	36.394791
1457.403649	202241.773712	36.399808
1459.130598	202573.354073	36.404826
1460.386938	202911.806763	36.409844
1461.902602	203247.056509	36.414861
1463.723581	203583.057069	36.419879
1464.798185	203933.619364	36.424896
1466.492489	204272.843691	36.429914
1467.791578	204622.826031	36.434932
1469.144385	204980.216226	36.439949
1470.441919	205323.472579	36.444967
1471.765143	205685.899088	36.449984
1473.224904	206049.091901	36.455002
1474.362889	206421.100966	36.460020
1475.946950	206788.238214	36.465037
1477.564705	207146.915054	36.470055
1478.490750	207516.158300	36.475072
1480.624657	207887.590153	36.480090
1482.016198	208256.505691	36.485108
1484.083229	208602.696253	36.490125
1485.831933	208965.524382	36.495143
1487.748147	209333.227715	36.500160
1489.739210	209669.721533	36.505178
1491.714247	210003.324240	36.510196
1493.415931	210351.398529	36.515213
1495.143333	210687.787783	36.520231
1496.165539	211026.047626	36.525248
1497.914953	211351.286919	36.530266
1499.540318	211701.995204	36.535284
1500.912743	212048.835782	36.540301
1502.209270	212388.172925	36.545319
1503.530631	212737.335784	36.550336
1504.881308	213073.212631	36.555354
1506.298819	213423.378115	36.560372
1507.648140	213773.734046	36.565389
1508.868447	214126.068297	36.570407
1510.151576	214483.371341	36.575424
1511.831778	214830.730394	36.580442
1513.053474	215190.103534	36.585460
1514.726970	215552.984197	36.590477
1517.157400	215883.765213	36.595495
1519.012117	216229.754437	36.600512
1521.371448	216545.869686	36.605530
1523.747273	216874.275790	36.610548
1525.507958	217183.838134	36.615565
1527.225372	217496.938952	36.620583
1528.689539	217809.447795	36.625600
1530.156751	218113.626518	36.630618
1531.983029	218413.378141	36.635636
1533.024865	218748.665945	36.640653
1534.277704	219087.475647	36.645671
1535.774012	219380.909821	36.650688
1537.371412	219658.784162	36.655706
1538.960878	219945.448477	36.660724
1540.167328	220236.901225	36.665741
1541.400105	220524.388206	36.670759
1542.490936	220827.087986	36.675776
1543.710143	221137.056819	36.680794
1544.963700	221448.874967	36.685812
1545.872727	221773.806226	36.690829
1547.352058	222091.100361	36.695847
1548.265052	222434.294862	36.700864
1549.860340	222771.433875	36.705882
1551.061493	223127.155350	36.710900
1552.082377	223480.748864	36.715917
1553.734448	223840.893493	36.720935
1554.889536	224206.912724	36.725952
1556.442809	224581.248968	36.730970
1557.557485	224946.972384	36.735988
1558.829318	225333.879704	36.741005
1560.429136	225711.031117	36.746023
1561.626039	226117.333449	36.751040
1563.015482	226513.216560	36.756058
1564.482414	226922.931140	36.761076
1565.892867	227340.632063	36.766093
1567.900081	227746.729066	36.771111
1569.597058	228159.609854	36.776128
1571.457431	228560.653621	36.781146
1572.950748	228974.891502	36.786164
1574.504856	229390.466791	36.791181
1576.343958	229802.084376	36.796199
1578.232830	230197.006615	36.801216
1580.512983	230595.903817	36.806234
1583.025197	230991.334531	36.811252
1584.615748	231389.230579	36.816269
1586.494353	231770.797881	36.821287
1588.036251	232158.975443	36.826304
1590.062136	232536.659286	36.831322
1592.613992	232892.386413	36.836340
1595.292730	233242.276423	36.841357
1596.864190	233602.562079	36.846375
1598.517414	233948.635611	36.851392
1599.960288	234295.252769	36.856410
1601.473904	234643.992646	36.861428
1603.420092	234995.938338	36.866445
1604.742802	235342.526758	36.871463
1606.479378	235692.857512	36.876480
1608.635421	236005.397926	36.881498
1611.148775	236322.578978	36.886516
1612.779627	236648.518069	36.891533
1614.276943	236973.489200	36.896551
1615.778903	237301.203528	36.901568
1616.897677	237622.682264	36.906586
1618.076811	237962.237718	36.911604
1619.191222	238307.875564	36.916621
1620.538956	238646.870806	36.921639
1621.480610	239005.747546	36.926656
1622.718700	239358.580873	36.931674
1624.377393	239719.600780	36.936692
1625.050308	240100.090373	36.941709
1626.588582	240467.786868	36.946727
1628.290578	240860.986141	36.951744
1629.552220	241253.624024	36.956762
1630.621154	241635.168268	36.961780
1632.295646	242024.919342	36.966797
1634.065779	242427.356420	36.971815
1635.594768	242830.418375	36.976832
1636.903531	243234.787595	36.981850
1638.876958	243638.437607	36.986868
1639.782260	244019.352103	36.991885
1641.547858	244415.874175	36.996903
1642.950644	244820.280966	37.001920
1644.189200	245222.226070	37.006938
1646.170054	245617.901208	37.011956
1647.596193	246023.271050	37.016973
1649.704157	246402.236474	37.021991
1651.473329	246805.746837	37.027008
1653.094498	247216.445821	37.032026
1654.992234	247608.606125	37.037044
1656.900375	248004.473956	37.042061
1659.240926	248391.989165	37.047079
1661.641239	248772.788465	37.052096
1663.453193	249158.080360	37.057114
1665.610474	249534.297294	37.062132
1667.046438	249921.227175	37.067149
1669.579248	250276.933034	37.072167
1672.065850	250626.956524	37.077184
1673.773869	250990.369726	37.082202
1675.406786	251335.149735	37.087220
1676.845790	251704.247503	37.092237
1678.834061	252045.387209	37.097255
1680.068951	252412.766432	37.102272
1681.210590	252787.807680	37.107290
1683.016828	253150.367628	37.112308
1684.542827	253521.890730	37.117325
1686.228831	253891.304428	37.122343
1687.742212	254268.113838	37.127360
1688.772947	254651.379611	37.132378
1690.245414	255034.927968	37.137396
1691.791335	255435.027212	37.142413
1693.612529	255828.501519	37.147431
1695.464274	256225.146285	37.152448
1696.763462	256622.924263	37.157466
1698.334333	257025.661745	37.162484
1700.087104	257435.659895	37.167501
1702.020626	257833.663193	37.172519
1703.694956	258229.118350	37.177536
1705.027960	258653.081789	37.182554
1706.586269	259056.100981	37.187572
1708.186672	259483.576559	37.192589
1709.978583	259897.607430	37.197607
1711.986169	260327.860616	37.202624
1713.452139	260741.742166	37.207642
1714.942291	261166.365214	37.212660
1716.632441	261608.534076	37.217677
1719.348760	262017.991157	37.222695
1721.698347	262415.645565	37.227712
1723.642660	262817.685551	37.232730
1725.702014	263218.131311	37.237748
1727.411727	263621.378391	37.242765
1728.758754	264026.107966	37.247783
1730.458305	264423.132546	37.252800
1731.771322	264834.522959	37.257818
1733.531223	265253.688641	37.262836
1735.122761	265666.480353	37.267853
1736.606459	266085.792852	37.272871
1738.580954	266500.324125	37.277888
1739.771764	266928.931245	37.282906
1741.881536	267337.215671	37.287924
1742.656814	267769.650572	37.292941
1744.433317	268198.845372	37.297959
1745.989320	268634.706472	37.302976
1747.720548	269079.352905	37.307994
1749.705297	269521.416533	37.313012
1751.205199	269960.079798	37.318029
1752.762021	270409.046673	37.323047
1754.307323	270842.976400	37.328064
1756.049795	271275.983798	37.333082
1758.350733	271690.912910	37.338100
1760.567576	272102.095809	37.343117
1762.530129	272511.262678	37.348135
1764.396397	272919.682860	37.353152
1766.241834	273333.643693	37.358170
1768.724489	273721.486057	37.363188
1770.390228	274141.318061	37.368205
1771.907894	274531.707013	37.373223
1773.333554	274939.689145	37.378240
1775.185542	275352.756668	37.383258
1777.366943	275762.339587	37.388276
1779.170595	276169.113940	37.393293
1780.834772	276586.833696	37.398311
1782.449436	277003.214577	37.403328
1784.181067	277419.727716	37.408346
1785.814189	277840.015909	37.413364
1787.515353	278252.518955	37.418381
1789.339922	278679.225898	37.423399
1791.818260	279084.460527	37.428416
1794.486982	279487.173401	37.433434
1796.963216	279886.691306	37.438452
1799.535251	280271.180015	37.443469
1802.518275	280632.001561	37.448487
1804.722519	280975.094019	37.453504
1806.789112	281340.638363	37.458522
1808.918715	281691.921195	37.463540
1810.224470	282039.682017	37.468557
1811.952978	282391.893577	37.473575
1813.889560	282750.267912	37.478592
1815.860209	283102.183878	37.483610
1817.349367	283458.954355	37.488628
1819.394566	283801.711987	37.493645
1820.877996	284159.624954	37.498663
1822.630218	284508.271936	37.503680
1824.332479	284883.369061	37.508698
1825.720363	285226.562771	37.513716
1827.553855	285602.830269	37.518733
1828.685539	285980.152962	37.523751
1829.995951	286363.134902	37.528768
1831.508103	286753.651881	37.533786
1833.098164	287150.962320	37.538804
1834.366360	287551.449284	37.543821
1836.001388	287961.424981	37.548839
1837.530297	288369.435816	37.553856
1838.814110	288800.244902	37.558874
1840.447885	289233.128273	37.563892
1842.266600	289660.823336	37.568909
1843.620463	290105.231202	37.573927
1845.243145	290557.086059	37.578944
1846.709788	291018.490208	37.583962
1848.776402	291466.229680	37.588980
1850.892978	291926.964010	37.593997
1852.674975	292381.478307	37.599015
1854.782553	292836.216355	37.604032
1856.887073	293304.033978	37.609050
1859.028221	293756.045197	37.614068
1861.575837	294192.138096	37.619085
1863.766985	294643.756583	37.624103
1865.690668	295075.784014	37.629120
1867.389157	295523.492944	37.634138
1869.817537	295957.287482	37.639156
1871.511961	296391.125717	37.644173
1873.461853	296822.303816	37.649191
1875.590317	297237.220828	37.654208
1877.239312	297678.554005	37.659226
1878.696190	298123.676133	37.664244
1880.679900	298556.873421	37.669261
1882.328970	298982.352456	37.674279
1883.914461	299397.655577	37.679296
1885.371182	299820.724727	37.684314
1886.733829	300256.405048	37.689332
1888.834030	300694.221650	37.694349
1890.586893	301124.195141	37.699367
1892.400903	301559.515479	37.704384
1894.051983	302010.353296	37.709402
1895.524083	302464.850436	37.714420
1897.462528	302921.985610	37.719437
1899.226998	303392.226860	37.724455
1901.301782	303846.414185	37.729472
1903.100459	304322.206905	37.734490
1904.727951	304785.911229	37.739508
1906.710675	305260.500204	37.744525
1908.435549	305747.395816	37.749543
1910.318404	306222.173890	37.754560
1912.184843	306710.843763	37.759578
1914.244218	307196.126595	37.764596
1916.397588	307684.692524	37.769613
1918.154788	308179.543179	37.774631
1919.976263	308673.770728	37.779648
1921.871518	309183.728219	37.784666
1923.244088	309688.258327	37.789684
1925.573007	310194.074342	37.794701
1927.021344	310712.679688	37.799719
1929.659687	311204.699323	37.804736
1931.615370	311717.017641	37.809754
1933.889467	312223.439090	37.814772
1936.536096	312726.189481	37.819789
1938.641592	313224.048940	37.824807
1940.771882	313718.853715	37.829824
1943.006278	314230.550181	37.834842
1944.532600	314732.507690	37.839860
1946.424996	315227.849607	37.844877
1948.278239	315733.656621	37.849895
1949.948602	316251.831376	37.854912
1952.010719	316754.295459	37.859930
1953.790835	317282.373083	37.864948
1955.785969	317785.755003	37.869965
1957.435788	318319.280320	37.874983
1959.153689	318847.965712	37.880000
1961.162148	319363.369686	37.885018
1963.119156	319896.907905	37.890036
1965.083602	320428.612443	37.895053
1967.150584	320957.959727	37.900071
1969.145040	321495.363727	37.905088
1971.189648	322029.555732	37.910106
1973.008737	322567.919349	37.915124
1975.237077	323099.507567	37.920141
1977.478266	323637.969952	37.925159
1979.620081	324155.700556	37.930176
1982.334295	324676.251871	37.935194
1984.262157	325193.653817	37.940212
1986.819894	325708.052676	37.945229
1988.352738	326234.575262	37.950247
1990.325118	326745.177762	37.955264
1991.867695	327276.208866	37.960282
1993.740560	327795.374879	37.965300
1995.935298	328321.287069	37.970317
1997.806259	328848.746072	37.975335
1999.632028	329365.925723	37.980352
2001.415217	329894.430660	37.985370
2003.713896	330440.108725	37.990388
2006.189012	330956.150982	37.995405
2007.628080	331489.090089	38.000423
2009.852893	332012.678636	38.005440
2012.037379	332527.053683	38.010458
2014.558914	333019.967587	38.015476
2016.592085	333508.845442	38.020493
2018.412126	334013.594901	38.025511
2019.803006	334506.631894	38.030528
2021.927842	335008.986105	38.035546
2023.556574	335504.462289	38.040564
2025.746769	336005.755500	38.045581
2027.689677	336521.909468	38.050599
2029.424765	337038.321239	38.055616
2030.998258	337557.419981	38.060634
2032.555062	338084.410627	38.065652
2034.979307	338606.353179	38.070669
2036.918231	339143.346886	38.075687
2038.722104	339685.636933	38.080704
2040.727023	340232.228282	38.085722
2042.533980	340780.090190	38.090740
2044.425229	341329.023532	38.095757
2046.333979	341896.375078	38.100775
2048.304171	342456.349244	38.105792
2050.467931	343019.635237	38.110810
2052.255676	343609.474644	38.115828
2054.870442	344162.545599	38.120845
2057.056342	344736.493050	38.125863
2059.261028	345301.877379	38.130880
2061.516529	345864.023284	38.135898
2064.095941	346438.164006	38.140916
2067.078815	346976.649318	38.145933
2069.868947	347526.200059	38.150951
2072.686501	348050.056632	38.155968
2075.537025	348571.846096	38.160986
2077.554895	349097.777185	38.166004
2080.252487	349608.515247	38.171021
2082.110067	350124.335207	38.176039
2084.226088	350632.214135	38.181056
2086.531072	351144.319249	38.186074
2088.434446	351655.114606	38.191092
2090.968048	352140.195067	38.196109
2093.939270	352634.180727	38.201127
2095.939463	353126.697549	38.206144
2098.428730	353614.712447	38.211162
2100.198202	354110.631151	38.216180
2102.271183	354588.909137	38.221197
2104.141979	355077.568010	38.226215
2106.662572	355550.051771	38.231232
2108.696176	356038.342691	38.236250
2109.859109	356536.236464	38.241268
2111.534935	357020.490017	38.246285
2113.247935	357535.610668	38.251303
2114.877196	358054.164064	38.256320
2116.955270	358584.460079	38.261338
2118.060838	359105.471888	38.266356
2119.931304	359639.112281	38.271373
2121.571043	360185.824692	38.276391
2123.126026	360754.692550	38.281408
2125.004944	361323.498660	38.286426
2126.621992	361907.435278	38.291444
2128.647160	362477.976506	38.296461
2131.127684	363057.770001	38.301479
2133.074641	363643.681098	38.306496
2135.351671	364226.814242	38.311514
2137.394042	364825.731171	38.316532
2139.100233	365413.836965	38.321549
2141.594543	366005.557578	38.326567
2143.921005	366604.577135	38.331584
2145.814895	367208.782908	38.336602
2147.746820	367806.174489	38.341620
2149.947263	368409.904257	38.346637
2152.412293	369008.025348	38.351655
2154.408833	369580.798511	38.356672
2156.538466	370162.012517	38.361690
2158.178470	370745.758703	38.366708
2160.372286	371332.422108	38.371725
2162.739559	371914.659391	38.376743
2164.833066	372503.501621	38.381760
2167.166022	373094.982952	38.386778
2169.240102	373679.294456	38.391796
2172.199023	374258.326705	38.396813
2174.423964	374832.322624	38.401831
2176.730294	375426.685891	38.406848
2179.297178	375997.562745	38.411866
2181.202309	376590.349503	38.416884
2183.499273	377176.873439	38.421901
2185.195787	377775.228131	38.426919
2187.270568	378364.710211	38.431936
2189.618427	378973.510642	38.436954
2191.418791	379582.669725	38.441972
2193.358120	380188.827960	38.446989
2195.660483	380808.100740	38.452007
2197.610468	381429.296750	38.457024
2200.326565	382046.804421	38.462042
2201.920734	382680.815285	38.467060
2203.866591	383306.388508	38.472077
2206.072192	383952.469283	38.477095
2208.035901	384592.999379	38.482112
2210.157148	385241.908072	38.487130
2211.929392	385899.278668	38.492148
2214.656292	386546.235269	38.497165
2216.987668	387218.773651	38.502183
2219.140959	387870.792576	38.507200
2221.393406	388523.567465	38.512218
2223.636089	389196.686727	38.517236
2225.963149	389877.052883	38.522253
2228.192250	390550.677432	38.527271
2230.239180	391226.345335	38.532288
2232.710736	391904.082648	38.537306
2234.866773	392575.672354	38.542324
2237.172008	393256.778337	38.547341
2239.365515	393927.115232	38.552359
2241.811105	394623.451009	38.557376
2244.743918	395286.690337	38.562394
2246.944422	395965.192293	38.567412
2249.372620	396638.977685	38.572429
2252.032839	397308.857034	38.577447
2253.796582	397982.899057	38.582464
2256.412752	398658.583685	38.587482
2258.563712	399339.828794	38.592500
2261.025296	400009.070707	38.597517
2263.500738	400681.132904	38.602535
2265.650657	401352.092921	38.607552
2268.297944	402024.196419	38.612570
2270.918652	402679.210012	38.617588
2273.689342	403329.698698	38.622605
2277.072381	403969.809177	38.627623
2279.320719	404602.415733	38.632640
2282.185654	405222.009533	38.637658
2284.911986	405849.390576	38.642676
2287.257225	406464.963493	38.647693
2289.746460	407062.789734	38.652711
2291.726616	407687.085527	38.657728
2294.308353	408281.424324	38.662746
2296.203168	408897.853016	38.667764
2297.974477	409520.063930	38.672781
2300.275980	410129.202716	38.677799
2302.585055	410747.369723	38.682816
2304.510198	411355.681639	38.687834
2306.681882	411970.828652	38.692852
2308.490013	412580.373061	38.697869
2310.647122	413172.773820	38.702887
2312.229700	413790.584842	38.707904
2314.761987	414392.394119	38.712922
2316.788819	414997.287138	38.717940
2318.274907	415622.744905	38.722957
2320.430998	416252.888583	38.727975
2322.205718	416893.792657	38.732992
2324.740235	417519.334712	38.738010
2326.873032	418174.506624	38.743028
2328.859454	418830.648196	38.748045
2331.062145	419493.244955	38.753063
2332.769109	420159.046341	38.758080
2335.272014	420849.918544	38.763098
2337.576048	421540.323499	38.768116
2339.273519	422233.493674	38.773133
2341.690106	422932.247612	38.778151
2343.826348	423643.560929	38.783168
2346.194225	424351.827811	38.788186
2349.045968	425062.930894	38.793204
2351.577010	425785.104290	38.798221
2354.021186	426495.979784	38.803239
2356.013990	427224.477656	38.808256
2358.577687	427949.669380	38.813274
2360.897851	428672.753142	38.818292
2363.154028	429402.963737	38.823309
2365.244708	430155.554933	38.828327
2367.946815	430902.250047	38.833344
2370.061942	431639.906968	38.838362
2372.695490	432388.287282	38.843380
2375.118546	433147.763600	38.848397
2377.672219	433891.452037	38.853415
2379.778894	434648.704471	38.858432
2382.099398	435425.685979	38.863450
2384.467217	436180.516544	38.868468
2387.192547	436946.700559	38.873485
2389.785073	437700.431377	38.878503
2392.727158	438460.455506	38.883520
2395.425977	439210.626539	38.888538
2398.329140	439954.615813	38.893556
2400.862001	440693.075567	38.898573
2403.761822	441436.965322	38.903591
2406.374852	442174.097576	38.908608
2409.088287	442909.164773	38.913626
2411.938313	443636.747507	38.918644
2414.480914	444361.726161	38.923661
2417.180254	445067.936354	38.928679
2420.041669	445797.114577	38.933696
2422.759219	446486.733039	38.938714
2424.960336	447188.605985	38.943732
2427.413341	447902.048534	38.948749
2429.894458	448598.517661	38.953767
2432.400982	449296.426643	38.958784
2434.802123	449999.539723	38.963802
2437.025642	450704.732481	38.968820
2439.513441	451406.064742	38.973837
2441.816412	452116.507405	38.978855
2444.355523	452821.829657	38.983872
2446.588475	453523.082519	38.988890
2448.815508	454226.891660	38.993908
2450.932861	454944.246880	38.998925
2453.372837	455656.720054	39.003943
2455.779393	456375.898929	39.008960
2457.503533	457092.232905	39.013978
2460.215506	457821.523689	39.018996
2461.949843	458557.927056	39.024013
2463.862100	459298.824192	39.029031
2466.454584	460031.492847	39.034048
2468.629091	460760.159758	39.039066
2471.044564	461481.379878	39.044084
2473.154733	462207.022145	39.049101
2475.509729	462921.072714	39.054119
2478.195751	463652.783964	39.059136
2481.290221	464373.938040	39.064154
2483.744200	465093.705939	39.069172
2486.177787	465827.450109	39.074189
2488.822143	466545.111432	39.079207
2491.050933	467279.946551	39.084224
2493.752625	468006.337464	39.089242
2496.494639	468734.008164	39.094260
2498.778326	469479.058858	39.099277
2501.427410	470212.903984	39.104295
2503.941096	470971.399871	39.109312
2505.919279	471725.659606	39.114330
2508.511228	472485.446160	39.119348
2510.725511	473243.092283	39.124365
2513.301180	474003.578092	39.129383
2515.454218	474773.397842	39.134400
2518.351689	475536.596915	39.139418
2520.856012	476312.356559	39.144436
2523.717206	477089.590450	39.149453
2526.496835	477862.815055	39.154471
2529.310473	478630.395470	39.159488
2532.339631	479391.948725	39.164506
2535.814953	480137.892624	39.169524
2539.126572	480883.732035	39.174541
2542.093751	481623.790650	39.179559
2544.726240	482352.008105	39.184576
2546.961879	483094.399734	39.189594
2549.679708	483827.794535	39.194612
2551.866205	484579.221093	39.199629
2554.747858	485315.910405	39.204647
2556.960673	486058.990393	39.209664
2558.805245	486814.114889	39.214682
2560.974891	487574.150804	39.219700
2562.865692	488350.453846	39.224717
2565.510137	489130.131078	39.229735
2567.524009	489912.855785	39.234752
2569.559787	490721.685572	39.239770
2572.162939	491517.514303	39.244788
2574.425411	492337.334178	39.249805
2576.875409	493154.106645	39.254823
2579.086257	493972.141351	39.259840
2581.686022	494793.301935	39.264858
2584.507673	495621.551033	39.269876
2587.279569	496447.245260	39.274893
2590.217004	497276.706099	39.279911
2592.832505	498106.734330	39.284928
2595.626752	498938.003570	39.289946
2598.305986	499757.597992	39.294964
2601.467163	500599.266628	39.299981
2603.924401	501417.655894	39.304999
2606.663810	502236.512820	39.310016
2609.644753	503059.626458	39.315034
2612.149244	503875.465176	39.320052
2614.744525	504700.678458	39.325069
2617.141566	505521.596604	39.330087
2619.594996	506358.347503	39.335104
2621.957164	507198.398128	39.340122
2624.315847	508022.422987	39.345140
2626.721724	508870.547116	39.350157
2629.443855	509710.306321	39.355175
2633.124607	510526.623491	39.360192
2635.871054	511355.806684	39.365210
2639.104573	512176.801122	39.370228
2642.050595	512982.326867	39.375245
2644.395442	513765.835610	39.380263
2646.680817	514545.585724	39.385280
2648.996567	515331.037106	39.390298
2651.741775	516110.280422	39.395316
2654.294314	516912.192266	39.400333
2656.368460	517696.103075	39.405351
2658.899035	518493.855348	39.410368
2660.980199	519319.401468	39.415386
2663.516564	520131.678861	39.420404
2665.263016	520957.192329	39.425421
2667.768687	521796.993004	39.430439
2670.415061	522625.340138	39.435456
2673.022188	523480.998772	39.440474
2676.212114	524318.683076	39.445492
2679.124216	525168.252485	39.450509
2681.835403	526025.411495	39.455527
2684.399313	526883.552969	39.460544
2686.367119	527766.316661	39.465562
2688.790096	528633.696231	39.470580
2691.710624	529521.786966	39.475597
2694.163067	530410.606610	39.480615
2696.780599	531303.221657	39.485632
2699.113897	532208.766611	39.490650
2702.298554	533116.933465	39.495668
2704.654151	534029.509526	39.500685
2706.994744	534955.166786	39.505703
2709.984418	535874.064707	39.510720
2712.585741	536805.498819	39.515738
2715.715873	537732.608536	39.520756
2718.619254	538667.998006	39.525773
2721.299627	539599.338011	39.530791
2724.345782	540528.745361	39.535808
2727.089672	541468.052210	39.540826
2730.906962	542381.514575	39.545844
2734.812558	543278.002169	39.550861
2738.397507	544174.183734	39.555879
2742.042587	545046.156862	39.560896
2744.674490	545947.612824	39.565914
2747.431834	546828.271143	39.570932
2750.211399	547702.735112	39.575949
2752.876847	548572.737840	39.580967
2755.977286	549456.138365	39.585984
2758.021240	550355.392736	39.591002
2760.883922	551219.815598	39.596020
2763.584152	552109.244061	39.601037
2766.364208	552986.235959	39.606055
2769.142704	553872.972347	39.611072
2771.481795	554764.447479	39.616090
2773.697110	555666.538097	39.621108
2776.584679	556564.436747	39.626125
2778.649993	557475.123922	39.631143
2781.553936	558385.660418	39.636160
2784.334075	559291.633303	39.641178
2787.185314	560193.061311	39.646196
2789.976500	561113.275596	39.651213
2792.980496	562031.933660	39.656231
2795.917477	562949.785085	39.661248
2798.861306	563858.329801	39.666266
2801.350567	564772.912839	39.671284
2804.021502	565701.512366	39.676301
2806.542280	566626.856551	39.681319
2809.840449	567551.051868	39.686336
2812.849939	568460.769297	39.691354
2815.891348	569375.889017	39.696372
2818.703708	570283.099970	39.701389
2821.806594	571203.198888	39.706407
2825.006839	572095.057657	39.711424
2827.917730	573010.540103	39.716442
2830.800319	573868.800819	39.721460
2833.472845	574729.095254	39.726477
2836.319218	575593.115540	39.731495
2839.465577	576436.605691	39.736512
2841.906872	577300.675406	39.741530
2844.583988	578148.191288	39.746548
2847.486643	579008.855331	39.751565
2849.604642	579883.985411	39.756583
2853.107118	580743.927901	39.761600
2855.656027	581622.574963	39.766618
2858.676700	582495.815412	39.771636
2860.937038	583377.894934	39.776653
2863.434720	584274.713663	39.781671
2866.770306	585162.302764	39.786688
2869.072208	586063.684822	39.791706
2871.928588	586952.124561	39.796724
2874.789931	587868.168530	39.801741
2877.354231	588790.958608	39.806759
2880.463106	589710.029136	39.811776
2883.321615	590644.756767	39.816794
2885.994358	591574.931788	39.821812
2888.760913	592500.107944	39.826829
2891.230291	593457.979079	39.831847
2894.390941	594397.872746	39.836864
2897.166628	595367.712553	39.841882
2899.300581	596332.669452	39.846900
2902.093420	597307.505527	39.851917
2904.546583	598301.047622	39.856935
2907.605617	599286.542297	39.861952
2910.240688	600293.054850	39.866970
2913.566890	601292.806299	39.871988
2916.091655	602309.926501	39.877005
2918.583683	603339.577667	39.882023
2922.120097	604374.970443	39.887040
2925.136748	605404.699387	39.892058
2927.604878	606426.218056	39.897076
2930.816572	607463.035310	39.902093
2933.738639	608512.915628	39.907111
2936.345131	609552.843646	39.912128
2939.070650	610611.266777	39.917146
2942.020132	611665.650978	39.922164
2945.526156	612718.343009	39.927181
2948.469518	613777.030396	39.932199
2951.817337	614821.096864	39.937216
2955.497143	615873.410871	39.942234
2958.855150	616921.777593	39.947252
2962.768977	617944.504279	39.952269
2965.476062	618994.380570	39.957287
2968.456804	620029.564566	39.962304
2971.574004	621056.730439	39.967322
2974.415475	622102.236419	39.972340
2977.300100	623141.037923	39.977357
2979.934778	624174.833974	39.982375
2983.227828	625216.415887	39.987392
2986.216251	626259.245936	39.992410
2988.880311	627293.435987	39.997428
2992.131889	628335.869827	40.002445
2994.540917	629399.916279	40.007463
2997.278858	630442.377964	40.012480
3000.328308	631502.960887	40.017498
3002.914176	632580.439348	40.022516
3006.177093	633635.279774	40.027533
3009.244536	634693.590394	40.032551
3012.310299	635747.900729	40.037568
3015.516564	636812.960921	40.042586
3018.223265	637866.267162	40.047604
3021.544823	638929.743176	40.052621
3024.582116	639976.492322	40.057639
3027.854123	641007.331541	40.062656
3030.684548	642022.925848	40.067674
3033.341900	643037.200889	40.072692
3036.565069	644046.742970	40.077709
3039.225960	645070.290569	40.082727
3042.014576	646102.040715	40.087744
3044.788848	647139.870195	40.092762
3047.008927	648193.188480	40.097780
3050.112214	649240.866763	40.102797
3052.843686	650309.231129	40.107815
3055.947833	651369.944061	40.112832
3059.009317	652431.597460	40.117850
3062.383953	653509.577856	40.122868
3065.571992	654585.927219	40.127885
3068.334520	655681.458047	40.132903
3071.221190	656766.635419	40.137920
3074.647638	657863.855183	40.142938
3076.747739	658973.122660	40.147956
3079.875638	660077.961207	40.152973
3082.896263	661206.440142	40.157991
3086.711960	662322.858089	40.163008
3089.859466	663450.805277	40.168026
3092.350871	664586.194203	40.173044
3095.562152	665721.827461	40.178061
3098.153827	666875.838629	40.183079
3100.945788	668030.672133	40.188096
3103.580206	669201.956624	40.193114
3106.466770	670395.387526	40.198132
3109.430995	671585.273074	40.203149
3112.614323	672786.657793	40.208167
3115.702213	673985.120277	40.213184
3118.838200	675186.354469	40.218202
3122.089722	676409.037488	40.223220
3125.008347	677617.897475	40.228237
3128.074500	678847.645710	40.233255
3131.236815	680069.562557	40.238272
3135.148233	681295.515687	40.243290
3138.102452	682523.847719	40.248308
3142.022853	683748.030775	40.253325
3145.746939	684960.511032	40.258343
3149.866838	686151.959048	40.263360
3154.234022	687338.691618	40.268378
3157.839399	688517.402024	40.273396
3161.692908	689683.756664	40.278413
3165.253153	690852.837151	40.283431
3168.446792	692013.389904	40.288448
3171.461361	693164.444095	40.293466
3174.174057	694324.527469	40.298484
3177.474935	695476.326389	40.303501
3180.477344	696645.482605	40.308519
3183.160022	697791.874352	40.313536
3186.194210	698956.801066	40.318554
3189.635470	700132.809232	40.323572
3192.588214	701294.612650	40.328589
3196.276202	702450.340856	40.333607
3199.715478	703602.289361	40.338624
3203.302908	704747.668353	40.343642
3205.839424	705906.446072	40.348660
3209.503304	707057.649303	40.353677
3212.652686	708210.368358	40.358695
3215.971358	709359.437750	40.363712
3218.970161	710524.052846	40.368730
3221.711657	711678.797846	40.373748
3224.718336	712841.114125	40.378765
3228.079811	714003.657782	40.383783
3230.972123	715171.414416	40.388800
3234.276514	716331.617615	40.393818
3237.214512	717494.739170	40.398836
3240.165069	718622.029855	40.403853
3243.237834	719757.705239	40.408871
3246.211119	720893.687337	40.413888
3249.320418	722028.848768	40.418906
3251.774038	723193.232806	40.423924
3254.812658	724344.651203	40.428941
3257.766221	725516.781427	40.433959
3260.773901	726672.377051	40.438976
3263.659616	727861.678478	40.443994
3266.847081	729062.120418	40.449012
3269.740110	730260.062906	40.454029
3273.077160	731476.672470	40.459047
3276.030887	732697.656586	40.464064
3279.323047	733922.695918	40.469082
3282.393417	735168.468777	40.474100
3285.860796	736410.872852	40.479117
3289.130962	737662.790018	40.484135
3292.390738	738914.315065	40.489152
3295.625506	740166.782119	40.494170
3298.665894	741438.421134	40.499188
3302.597649	742700.238355	40.504205
3305.610860	743981.435424	40.509223
3309.247923	745267.892196	40.514240
3312.371047	746545.102465	40.519258
3316.338771	747820.042006	40.524276
3319.956894	749108.974661	40.529293
3323.446323	750393.329236	40.534311
3326.436746	751686.716697	40.539328
3329.951555	752970.294046	40.544346
3333.470615	754267.741955	40.549364
3336.641625	755562.762899	40.554381
3340.757023	756854.159168	40.559399
3343.865712	758151.163939	40.564416
3347.273086	759442.730453	40.569434
3349.762096	760749.089423	40.574452
3353.330421	762057.307437	40.579469
3356.409216	763387.072227	40.584487
3359.848095	764702.672939	40.589504
3363.989888	766019.598296	40.594522
3366.876989	767350.953071	40.599540
3369.656615	768678.990783	40.604557
3373.327131	770025.516006	40.609575
3375.961879	771368.626041	40.614592
3379.277570	772716.144558	40.619610
3382.702507	774076.267504	40.624628
3386.101368	775428.530363	40.629645
3389.441003	776798.425772	40.634663
3392.303166	778189.644898	40.639680
3395.914301	779559.122973	40.644698
3399.221161	780953.370687	40.649716
3402.719125	782322.785727	40.654733
3406.450506	783697.003347	40.659751
3409.704173	785091.880881	40.664768
3413.410027	786477.095018	40.669786
3417.117598	787867.677801	40.674804
3420.755042	789245.550064	40.679821
3424.406008	790624.573454	40.684839
3427.837234	792010.223661	40.689856
3431.494478	793386.550295	40.694874
3434.754250	794766.982984	40.699892
3438.171685	796152.797837	40.704909
3441.532642	797536.437570	40.709927
3444.670736	798940.495452	40.714944
3447.783317	800335.807078	40.719962
3451.096692	801737.898814	40.724980
3454.444107	803135.101529	40.729997
3458.126560	804517.047723	40.735015
3461.084249	805914.574994	40.740020
3464.784149	807250.967106	40.745024
3467.925963	808527.648078	40.750029
3471.187303	809775.455646	40.755034
3474.560389	810927.195090	40.760039
3477.156251	812020.825559	40.765044
3480.872460	813029.616070	40.770048
3483.603742	813993.663521	40.775053
3486.512167	814878.082828	40.780058
3489.229584	815693.882658	40.785063
3491.468992	816457.385999	40.790068
3493.925161	817147.156846	40.795072
3496.244092	817771.351212	40.800077
3498.077207	818326.619653	40.805082
3500.539836	818825.908420	40.810087
3502.002964	819281.388506	40.815092
3503.637470	819669.196198	40.820096
3505.242420	820024.110909	40.825101
3506.327677	820322.835500	40.830106
3507.820015	820580.046424	40.835111
3509.000461	820793.666094	40.840116
3510.299995	820975.415923	40.845120
3511.372494	821116.893704	40.850125
3512.505174	821210.619829	40.855130
3513.634727	821278.079308	40.860135
3514.609278	821317.243740	40.865140
3515.219886	821314.599546	40.870144
3516.239380	821303.964039	40.875149
3516.649735	821246.571171	40.880154
3517.713261	821166.618814	40.885159
3517.937248	821077.510614	40.890164
3518.747128	820954.162071	40.895168
3519.231059	820822.842937	40.900173
3519.661049	820664.528106	40.905178
3520.315404	820489.833806	40.910183
3520.686643	820320.954170	40.915188
3520.966072	820104.094159	40.920192
3521.393112	819885.930685	40.925197
3521.589400	819647.788172	40.930202
3521.851187	819406.397178	40.935207
3522.057707	819160.260546	40.940212
3522.144448	818894.807340	40.945216
3522.413278	818616.297587	40.950221
3522.723556	818348.779454	40.955226
3522.924580	818055.136859	40.960231
3522.547761	817768.183451	40.965236
3522.952257	817465.329819	40.970240
3523.139449	817169.790784	40.975245
3523.080476	816850.198526	40.980250
3523.246351	816529.819615	40.985255
3522.799789	816199.981382	40.990260
3523.148830	815880.911702	40.995264
3523.504205	815551.594323	41.000269
3523.285832	815224.069047	41.005274
3523.237099	814877.209810	41.010279
3523.101691	814549.686839	41.015284
3522.888988	814218.145603	41.020288
3523.043469	813888.583919	41.025293
3522.783320	813536.206090	41.030298
3523.171526	813192.076804	41.035303
3522.668798	812859.194246	41.040308
3522.874228	812511.534264	41.045312
3522.783317	812176.345981	41.050317
3522.426658	811835.356171	41.055322
3522.666886	811478.722600	41.060327
3522.665567	811143.615191	41.065332
3522.321597	810789.932008	41.070336
3522.415828	810448.160841	41.075341
3522.001432	810103.565828	41.080346
3522.125072	809757.394489	41.085351
3521.979615	809415.071863	41.090356
3521.830538	809072.683566	41.095360
3521.802414	808737.706601	41.100365
3521.686647	808394.151515	41.105370
3521.869788	808060.674488	41.110375
3521.296311	807722.699105	41.115380
3521.047879	807382.300582	41.120384
3520.809189	807042.814752	41.125389
3520.896808	806725.757532	41.130394
3520.992008	806396.233102	41.135399
3520.744105	806058.954809	41.140404
3520.637913	805732.569129	41.145408
3520.857481	805404.300022	41.150413
3520.300540	805072.956528	41.155418
3520.216084	804744.657007	41.160423
3519.878240	804424.817617	41.165428
3519.789803	804102.225061	41.170432
3519.704510	803781.725519	41.175437
3519.294345	803472.544274	41.180442
3519.740181	803150.456281	41.185447
3519.024034	802840.953887	41.190452
3519.341743	802526.901437	41.195456
3518.737251	802223.876268	41.200461
3518.655541	801924.724648	41.205466
3518.395308	801605.820472	41.210471
3518.506139	801321.180145	41.215476
3518.896851	801025.149227	41.220480
3518.482547	800719.966105	41.225485
3518.380720	800421.586736	41.230490
3518.544866	800111.669246	41.235495
3518.080361	799812.685708	41.240500
3517.906532	799521.541449	41.245504
3517.449638	799235.191691	41.250509
3517.509993	798947.370574	41.255514
3517.482677	798654.938894	41.260519
3517.179922	798391.005499	41.265524
3517.170140	798092.903339	41.270528
3516.948594	797818.235391	41.275533
3516.921258	797539.548737	41.280538
3516.808620	797263.761074	41.285543
3516.744906	796988.936162	41.290548
3516.575494	796710.043457	41.295552
3516.547579	796441.376324	41.300557
3516.427594	796169.866654	41.305562
3516.426890	795894.251819	41.310567
3516.408030	795635.371222	41.315572
3516.371759	795361.410558	41.320576
3516.326281	795094.216605	41.325581
3515.911192	794822.899800	41.330586
3516.037917	794562.826113	41.335591
3515.617927	794305.141117	41.340596
3515.380394	794045.894146	41.345600
3515.148119	793796.311387	41.350605
3515.149624	793536.613226	41.355610
3515.512023	793292.611263	41.360615
3515.155145	793033.002825	41.365620
3515.232841	792775.719727	41.370624
3515.256730	792536.953894	41.375629
3514.993500	792289.876940	41.380634
3514.899338	792038.342385	41.385639
3514.566448	791798.873657	41.390644
3514.329079	791549.506772	41.395648
3514.298567	791314.491184	41.400653
3514.236966	791084.140150	41.405658
3514.438346	790842.192487	41.410663
3513.649411	790604.871214	41.415668
3513.908766	790373.019132	41.420672
3513.643049	790150.287124	41.425677
3513.886363	789927.070896	41.430682
3513.586983	789700.497621	41.435687
3513.454410	789472.562754	41.440692
3513.137246	789248.778952	41.445696
3513.278602	789028.892911	41.450701
3512.887799	788817.442574	41.455706
3513.212582	788589.944359	41.460711
3512.739977	788392.747253	41.465716
3512.776282	788172.065679	41.470720
3512.766224	787957.971087	41.475725
3512.724952	787754.934397	41.480730
3512.642307	787544.722363	41.485735
3512.330489	787337.982826	41.490740
3512.265106	787126.428410	41.495744
3512.279025	786927.586443	41.500749
3512.146853	786735.940280	41.505754
3512.146059	786525.438851	41.510759
3512.154524	786315.273816	41.515764
3512.060449	786119.770182	41.520768
3511.894281	785918.914172	41.525773
3511.595302	785731.250923	41.530778
3511.907535	785534.189148	41.535783
3511.658394	785342.180733	41.540788
3511.440738	785150.456979	41.545792
3511.236436	784966.249065	41.550797
3511.088380	784785.616699	41.555802
3511.482187	784589.007148	41.560807
3510.959242	784412.607088	41.565812
3511.466468	784222.066421	41.570816
3511.139484	784043.215254	41.575821
3510.880999	783858.840293	41.580826
3511.010976	783677.740641	41.585831
3510.552152	783494.618927	41.590836
3510.505617	783327.310330	41.595840
3510.740937	783143.622323	41.600845
3510.612809	782975.236974	41.605850
3510.645351	782797.475803	41.610855
3510.014009	782633.198847	41.615860
3510.177132	782468.147409	41.620864
3510.340035	782301.468977	41.625869
3509.986047	782125.673472	41.630874
3509.917600	781957.943128	41.635879
3509.772959	781802.175325	41.640884
3509.961140	781634.739405	41.645888
3509.866315	781467.149585	41.650893
3509.613266	781321.228313	41.655898
3509.728744	781149.365500	41.660903
3509.676501	781004.093397	41.665908
3509.413950	780846.454914	41.670912
3509.438790	780696.686754	41.675917
3509.131224	780544.903964	41.680922
3508.895843	780386.906557	41.685927
3509.116679	780249.643355	41.690932
3508.936921	780097.141200	41.695936
3509.160436	779959.084776	41.700941
3508.968564	779812.532468	41.705946
3509.054784	779653.334157	41.710951
3508.903277	779526.255490	41.715956
3508.936976	779378.082453	41.720960
3508.969878	779236.992796	41.725965
3508.828464	779092.336782	41.730970
3508.907399	778940.259639	41.735975
3508.992859	778809.635186	41.740980
3508.610185	778661.319460	41.745984
3508.651732	778515.292929	41.750989
3508.461065	778385.198620	41.755994
3508.506746	778244.333637	41.760999
3508.443206	778100.186372	41.766004
3508.444174	777970.594371	41.771008
3508.434199	777834.406429	41.776013
3508.384973	777699.256057	41.781018
3508.372532	777560.602365	41.786023
3507.931770	777435.995992	41.791028
3507.964007	777295.262520	41.796032
3508.117601	777166.517002	41.801037
3507.795756	777053.353668	41.806042
3507.968498	776918.447475	41.811047
3507.581318	776789.046260	41.816052
3507.846373	776665.737652	41.821056
3508.027823	776549.628127	41.826061
3507.511401	776419.207908	41.831066
3507.504457	776302.584061	41.836071
3507.145485	776196.059612	41.841076
3507.188452	776078.242394	41.846080
3507.214819	775950.973396	41.851085
3507.265929	775845.951511	41.856090
3507.546240	775722.378288	41.861095
3507.144731	775603.592952	41.866100
3506.985906	775494.464985	41.871104
3507.221704	775382.512949	41.876109
3507.095454	775266.138457	41.881114
3507.280513	775144.885360	41.886119
3507.147094	775045.249397	41.891124
3506.811160	774929.938217	41.896128
3506.781395	774818.513832	41.901133
3506.581169	774731.637806	41.906138
3506.626332	774606.902833	41.911143
3506.701546	774507.471284	41.916148
3506.373442	774406.086077	41.921152
3506.574751	774303.627113	41.926157
3506.395221	774212.161858	41.931162
3506.523418	774099.370845	41.936167
3506.649847	774004.602280	41.941172
3506.609781	773901.931366	41.946176
3506.487506	773801.734945	41.951181
3506.373225	773704.441442	41.956186
3506.454912	773596.181157	41.961191
3506.464348	773497.830259	41.966196
3506.181254	773402.678356	41.971200
3506.249450	773292.987595	41.976205
3506.124801	773200.958917	41.981210
3506.180161	773107.126284	41.986215
3505.715727	773019.387112	41.991220
3505.926289	772936.854644	41.996224
3506.084896	772839.356834	42.001229
3505.967421	772757.024316	42.006234
3505.844436	772651.049614	42.011239
3505.992524	772569.163657	42.016244
3506.066294	772479.752944	42.021248
3505.924466	772377.520854	42.026253
3505.977160	772292.298144	42.031258
3505.995533	772200.972178	42.036263
3505.812198	772112.338355	42.041268
3505.519110	772025.150108	42.046272
3506.046356	771932.850072	42.051277
3505.901447	771853.566068	42.056282
3505.695563	771755.030420	42.061287
3505.694323	771674.489235	42.066292
3505.510895	771583.386010	42.071296
3505.530047	771498.061138	42.076301
3505.423035	771417.830204	42.081306
3505.499430	771339.784941	42.086311
3505.517728	771263.916065	42.091316
3505.306395	771176.901332	42.096320
3505.608062	771087.879465	42.101325
3505.365235	771023.776344	42.106330
3505.427528	770924.988234	42.111335
3505.370228	770844.841391	42.116340
3505.280683	770767.852108	42.121344
3505.172392	770685.642742	42.126349
3505.097202	770607.466989	42.131354
3505.249821	770537.973333	42.136359
3505.293195	770456.426119	42.141364
3504.981842	770387.451142	42.146368
3504.978847	770306.304092	42.151373
3504.573448	770242.073243	42.156378
3504.844379	770154.572613	42.161383
3504.735869	770089.995755	42.166388
3504.608953	770019.360901	42.171392
3504.622592	769949.244145	42.176397
3504.473553	769906.253764	42.181402
3504.622350	769831.777543	42.186407
3504.582092	769766.940221	42.191412
3504.474411	769703.394605	42.196416
3504.788051	769633.767306	42.201421
3504.515585	769569.853577	42.206426
3504.554909	769495.096413	42.211431
3504.886458	769435.220864	42.216436
3504.718550	769365.325688	42.221440
3504.724604	769296.583753	42.226445
3504.331343	769232.243580	42.231450
3504.380975	769155.904416	42.236455
3504.503818	769098.228865	42.241460
3504.047013	769043.014027	42.246464
3504.429547	768974.108334	42.251469
3504.077711	768915.228543	42.256474
3504.190852	768846.464742	42.261479
3504.294281	768784.256202	42.266484
3504.111940	768737.864199	42.271488
3504.056875	768675.878064	42.276493
3504.111560	768620.279869	42.281498
3504.165393	768562.710126	42.286503
3504.072229	768494.469976	42.291508
3504.012158	768452.146412	42.296512
3504.132294	768388.453320	42.301517
3503.890756	768339.703027	42.306522
3503.923575	768286.225129	42.311527
3503.993729	768224.165250	42.316532
3503.870617	768186.286156	42.321536
3503.982483	768131.857683	42.326541
3503.600235	768081.847547	42.331546
3504.011879	768021.060238	42.336551
3503.734731	767974.038420	42.341556
3503.527606	767920.153968	42.346560
3504.007192	767870.344996	42.351565
3503.576831	767823.051822	42.356570
3503.704897	767762.358549	42.361575
3503.811183	767713.448097	42.366580
3503.663168	767662.706409	42.371584
3503.698164	767614.743557	42.376589
3503.713541	767569.740944	42.381594
3503.511943	767516.296248	42.386599
3503.514239	767466.957762	42.391604
3503.586928	767427.169460	42.396608
3503.692609	767378.848383	42.401613
3503.092801	767334.340322	42.406618
3503.192262	767289.568571	42.411623
3503.325824	767253.515344	42.416628
3503.332673	767210.335717	42.421632
3503.423407	767160.832717	42.426637
3503.195756	767123.359815	42.431642
3503.115045	767074.771818	42.436647
3503.318278	767040.874884	42.441652
3503.391538	766998.915357	42.446656
3503.576900	766952.599330	42.451661
3503.237901	766902.672702	42.456666
3503.578290	766867.914340	42.461671
3503.321153	766823.543770	42.466676
3502.974071	766781.948242	42.471680
3503.338706	766743.093919	42.476685
3502.847669	766715.274791	42.481690
3503.089610	766676.588279	42.486695
3503.244019	766633.430223	42.491700
3502.670789	766597.293440	42.496704
3503.117723	766567.248377	42.501709
3503.141536	766532.639358	42.506714
3503.262887	766488.647908	42.511719
3503.501648	766452.819906	42.516724
3503.080775	766413.354234	42.521728
3503.176069	766363.795896	42.526733
3503.296520	766326.064277	42.531738
3503.211922	766287.281819	42.536743
3502.989726	766242.852722	42.541748
3503.185158	766199.882570	42.546752
3503.292895	766167.377782	42.551757
3503.396489	766126.788675	42.556762
3503.152456	766089.658370	42.561767
3503.167163	766046.322814	42.566772
3503.008575	766017.805263	42.571776
3503.252927	765972.853775	42.576781
3502.891228	765948.510636	42.581786
3502.655110	765893.186640	42.586791
3502.662364	765868.979471	42.591796
3502.778966	765841.648264	42.596800
3503.147451	765807.077527	42.601805
3502.748416	765777.612790	42.606810
3502.881559	765742.193238	42.611815
3503.217453	765705.754000	42.616820
3502.795197	765668.059440	42.621824
3503.122319	765623.042872	42.626829
3503.059212	765584.992736	42.631834
3502.857793	765558.699078	42.636839
3503.017318	765518.886257	42.641844
3502.793822	765481.650931	42.646848
3502.628994	765446.920149	42.651853
3502.619924	765428.186820	42.656858
3502.533224	765390.632619	42.661863
3502.713136	765361.711507	42.666868
3502.228314	765333.294556	42.671872
3502.922455	765298.519749	42.676877
3502.451070	765283.362995	42.681882
3502.710207	765251.913888	42.686887
3502.948770	765219.975009	42.691892
3502.786885	765189.926421	42.696896
3503.010225	765155.919010	42.701901
3502.869000	765123.943873	42.706906
3503.033745	765094.827019	42.711911
3502.753040	765056.465019	42.716916
3502.955696	765041.393610	42.721920
3502.861042	765002.507538	42.726925
3502.864957	764966.711230	42.731930
3502.573620	764933.034386	42.736935
3502.619361	764900.780869	42.741940
3502.711851	764872.118845	42.746944
3502.983618	764844.709053	42.751949
3502.441890	764819.603078	42.756954
3503.038447	764774.043822	42.761959
3502.737475	764741.255230	42.766964
3502.621163	764727.024812	42.771968
3502.750926	764684.648501	42.776973
3502.837672	764656.528984	42.781978
3502.459341	764637.805390	42.786983
3502.599313	764600.850771	42.791988
3502.527109	764578.871420	42.796993
3502.657857	764535.655866	42.801997
3502.686090	764517.850956	42.807002
3502.163116	764482.287327	42.812007
3502.475938	764461.871198	42.817012
3502.132445	764438.999397	42.822017
3502.245500	764412.797672	42.827021
3502.471419	764394.466709	42.832026
3502.137879	764369.571366	42.837031
3502.129212	764352.511804	42.842036
3502.161455	764318.187006	42.847041
3502.242531	764304.860055	42.852045
3502.368045	764282.304753	42.857050
3502.312541	764259.828605	42.862055
3502.508907	764246.778362	42.867060
3502.259458	764226.996923	42.872065
3502.298501	764203.913259	42.877069
3502.393309	764175.001634	42.882074
3502.128899	764166.465366	42.887079
3502.601514	764130.143813	42.892084
3502.245929	764120.044602	42.897089
3502.530423	764080.203490	42.902093
3502.278292	764060.569989	42.907098
3502.477268	764039.974282	42.912103
3502.314314	764015.789249	42.917108
3502.280720	763991.780010	42.922113
3502.303484	763971.163921	42.927117
3502.004830	763952.819942	42.932122
3502.139628	763933.171480	42.937127
3502.157478	763910.534227	42.942132
3502.305315	763894.631263	42.947137
3502.326745	763869.182473	42.952141
3502.079560	763844.665617	42.957146
3502.440647	763821.626187	42.962151
3502.297306	763793.837338	42.967156
3502.132809	763781.782872	42.972161
3502.208665	763756.127451	42.977165
3502.182307	763739.759809	42.982170
3502.470067	763706.721462	42.987175
3502.694213	763689.769863	42.992180
3502.231674	763664.153783	42.997185
3502.473244	763639.407548	43.002189
3502.130891	763624.275416	43.007194
3502.368823	763598.839248	43.012199
3502.679233	763569.347204	43.017204
3502.223081	763557.883037	43.022209
3502.162503	763513.065824	43.027213
3502.078023	763499.567542	43.032218
3502.107249	763484.176463	43.037223
3502.367241	763461.547159	43.042228
3502.193922	763451.762134	43.047233
3502.183732	763429.177380	43.052237
3502.039253	763423.678018	43.057242
3502.066243	763396.007497	43.062247
3502.146196	763365.122574	43.067252
3502.110158	763363.747802	43.072257
3502.301958	763339.008804	43.077261
3502.070571	763322.871400	43.082266
3502.236513	763303.364096	43.087271
3502.320948	763277.113824	43.092276
3501.810364	763258.359316	43.097281
3502.076200	763239.279190	43.102285
3501.930606	763223.719199	43.107290
3501.924618	763216.963873	43.112295
3501.972147	763192.445502	43.117300
3502.134294	763168.894460	43.122305
3502.205998	763153.446368	43.127309
3502.050783	763135.816448	43.132314
3501.965523	763123.501243	43.137319
3501.998480	763102.782452	43.142324
3501.782797	763076.235848	43.147329
3502.295563	763073.734655	43.152333
3502.076401	763058.334433	43.157338
3501.992909	763034.527653	43.162343
3502.191676	763010.328925	43.167348
3501.854893	763004.713078	43.172353
3502.091412	762977.499578	43.177357
3501.760373	762960.243532	43.182362
3501.924261	762949.070520	43.187367
3502.076628	762943.275157	43.192372
3502.030263	762914.135418	43.197377
3502.361671	762902.441464	43.202381
3502.219301	762879.383710	43.207386
3502.537241	762861.329723	43.212391
3502.093620	762831.860756	43.217396
3502.100522	762826.138661	43.222401
3502.460282	762798.904151	43.227405
3502.158819	762767.192045	43.232410
3502.363662	762758.921867	43.237415
3502.422000	762731.736924	43.242420
3502.399029	762717.092706	43.247425
3502.461436	762683.741867	43.252429
3502.056892	762669.160610	43.257434
3502.536451	762640.919319	43.262439
3502.562927	762617.290330	43.267444
3502.127718	762599.557458	43.272449
3502.311466	762580.489231	43.277453
3502.582038	762562.393035	43.282458
3502.199141	762531.334570	43.287463
3502.215919	762517.176610	43.292468
3501.722114	762488.996954	43.297473
3502.171272	762463.078150	43.302477
3501.905333	762463.714085	43.307482
3502.068852	762439.716639	43.312487
3502.076743	762421.071646	43.317492
3502.036060	762406.824330	43.322497
3502.094975	762369.625528	43.327501
3501.824395	762370.114270	43.332506
3502.161862	762359.355605	43.337511
3502.040612	762326.822699	43.342516
3501.591885	762324.677443	43.347521
3502.126718	762307.671396	43.352525
3502.083147	762273.645732	43.357530
3501.978572	762281.456212	43.362535
3502.145053	762259.825219	43.367540
3501.924660	762234.213565	43.372545
3501.830242	762222.391633	43.377549
3502.202280	762222.576897	43.382554
3501.964642	762192.084910	43.387559
3502.216423	762170.143621	43.392564
3502.079229	762155.566510	43.397569
3502.221518	762128.809436	43.402573
3502.169963	762117.325525	43.407578
3501.884193	762093.499871	43.412583
3501.911725	762072.187248	43.417588
3501.945782	762073.957430	43.422593
3502.059436	762058.598811	43.427597
3501.970095	762030.597222	43.432602
3502.072226	762023.231060	43.437607
3502.142770	762004.969284	43.442612
3501.759088	761978.693194	43.447617
3502.202456	761987.005334	43.452621
3501.904523	761952.231049	43.457626
3501.766398	761927.640591	43.462631
3502.059703	761913.287825	43.467636
3501.626667	761919.031955	43.472641
3501.488567	761882.652517	43.477645
3501.711838	761872.898549	43.482650
3501.691327	761864.319351	43.487655
3501.800831	761858.184958	43.492660
3501.785949	761857.398326	43.497665
3501.666036	761827.082711	43.502669
3501.848792	761830.406817	43.507674
3501.376035	761825.503118	43.512679
3501.817586	761815.022439	43.517684
3501.565337	761809.934312	43.522689
3501.759454	761787.557504	43.527693
3501.617768	761779.787457	43.532698
3501.492740	761777.785855	43.537703
3501.853402	761769.094234	43.542708
3501.739384	761749.431867	43.547713
3501.544501	761730.868002	43.552717
3501.472146	761723.481055	43.557722
3501.585366	761721.834683	43.562727
3501.847663	761717.253388	43.567732
3501.551041	761703.342997	43.572737
3501.665333	761683.100132	43.577741
3501.544554	761680.209913	43.582746
3501.345606	761682.166673	43.587751
3501.688892	761668.791727	43.592756
3501.565330	761679.910892	43.597761
3501.739423	761657.191717	43.602765
3501.298411	761641.726598	43.607770
3501.510624	761633.059352	43.612775
3501.652988	761630.668232	43.617780
3501.607060	761640.689420	43.622785
3501.599779	761629.690724	43.627789
3501.366854	761627.312292	43.632794
3501.769221	761591.335412	43.637799
3501.900077	761567.537902	43.642804
3501.692210	761584.639812	43.647809
3501.647644	761573.992491	43.652813
3501.725698	761560.019920	43.657818
3501.622405	761539.122034	43.662823
3501.800641	761530.361628	43.667828
3501.543486	761530.749545	43.672833
3501.570841	761519.498325	43.677837
3501.646466	761513.122610	43.682842
3501.412416	761498.412248	43.687847
3501.598395	761481.511324	43.692852
3501.674459	761475.776775	43.697857
3501.700747	761466.794764	43.702861
3502.299073	761472.072827	43.707866
3501.925596	761456.448181	43.712871
3501.997131	761425.260728	43.717876
3501.826725	761410.736993	43.722881
3501.783634	761380.554875	43.727885
3501.796022	761383.167396	43.732890
3501.505130	761382.771628	43.737895
3501.619834	761370.716486	43.742900
3501.577557	761354.642265	43.747905
3501.624396	761328.884715	43.752909
3501.965036	761325.720793	43.757914
3501.557920	761320.263289	43.762919
3501.635364	761312.111242	43.767924
3501.542742	761292.345488	43.772929
3501.682707	761280.532677	43.777933
3501.643840	761280.835203	43.782938
3501.603542	761284.936357	43.787943
3501.783360	761280.960387	43.792948
3501.807761	761267.982738	43.797953
3501.915845	761244.089312	43.802957
3501.594446	761241.281407	43.807962
3501.405922	761241.805985	43.812967
3501.888379	761224.510185	43.817972
3501.610202	761210.398514	43.822977
3501.923276	761191.552060	43.827981
3501.893745	761188.153270	43.832986
3501.811201	761178.251622	43.837991
3501.685043	761152.176744	43.842996
3501.966725	761155.435472	43.848001
3501.447918	761145.556543	43.853005
3501.869868	761129.849106	43.858010
3501.879333	761117.958944	43.863015
3501.864656	761099.561069	43.868020
3501.484130	761100.166716	43.873025
3501.602711	761090.725027	43.878029
3501.808324	761055.172760	43.883034
3501.408133	761063.378667	43.888039
3501.505673	761047.626006	43.893044
3501.253812	761051.416929	43.898049
3501.280180	761054.717891	43.903053
3501.646584	761052.338899	43.908058
3501.418386	761065.646832	43.913063
3501.415409	761042.905741	43.918068
3501.613334	761013.126309	43.923073
3501.665933	761007.691273	43.928077
3501.784020	760999.976157	43.933082
3501.530321	761009.489868	43.938087
3501.718086	760995.103471	43.943092
3501.560106	760984.276733	43.948097
3501.647019	760969.610964	43.953101
3501.893108	760955.313517	43.958106
3501.727962	760953.712979	43.963111
3501.736815	760934.916160	43.968116
3501.375032	760918.548484	43.973121
3501.408100	760911.044656	43.978125
3501.628288	760908.245792	43.983130
3501.602550	760904.648918	43.988135
3501.639902	760897.835019	43.993140
3501.491306	760880.297389	43.998145
3501.321296	760871.051113	44.003149
3501.684897	760851.702141	44.008154
3501.493898	760851.733828	44.013159
3501.905666	760857.980476	44.018164
3501.804728	760857.997281	44.023169
3501.633707	760817.967542	44.028173
3501.968315	760803.704515	44.033178
3501.222657	760813.743763	44.038183
3501.724567	760803.202382	44.043188
3501.593973	760802.780091	44.048193
3501.376466	760774.104359	44.053197
3501.680335	760767.246302	44.058202
3501.501580	760768.311961	44.063207
3501.559335	760753.107926	44.068212
3501.626465	760754.379621	44.073217
3501.398038	760746.820175	44.078221
3501.567830	760724.740243	44.083226
3501.536659	760728.396190	44.088231
3501.584021	760710.332449	44.093236
3501.684883	760713.374583	44.098241
3501.826059	760707.234025	44.103245
3501.832410	760695.491714	44.108250
3501.511036	760679.264842	44.113255
3501.741048	760663.538824	44.118260
3501.992884	760674.153427	44.123265
3501.535216	760664.017092	44.128269
3502.075382	760627.174184	44.133274
3501.833474	760624.698247	44.138279
3502.150853	760606.836311	44.143284
3501.866178	760586.903111	44.148289
3501.681196	760572.922849	44.153293
3501.926193	760561.584904	44.158298
3501.565836	760574.718200	44.163303
3501.742247	760543.263106	44.168308
3501.698674	760536.659594	44.173313
3501.911397	760516.446676	44.178317
3501.676870	760515.844204	44.183322
3501.671477	760504.596885	44.188327
3502.040424	760484.654075	44.193332
3501.908094	760484.577398	44.198337
3501.936149	760469.328365	44.203341
3502.035190	760440.204377	44.208346
3501.672116	760436.564354	44.213351
3501.697391	760434.340214	44.218356
3501.731333	760422.247573	44.223361
3501.817372	760395.197645	44.228365
3501.781224	760381.587119	44.233370
3501.672305	760396.307249	44.238375
3501.766305	760371.229342	44.243380
3501.541786	760357.748572	44.248385
3501.651605	760344.607216	44.253389
3501.872180	760331.102183	44.258394
3501.658217	760341.448876	44.263399
3501.759742	760330.430310	44.268404
3501.702026	760314.899124	44.273409
3501.737745	760307.295587	44.278413
3501.881272	760309.344111	44.283418
3501.433618	760298.070896	44.288423
3501.723190	760267.829363	44.293428
3501.487146	760258.099884	44.298433
3501.441562	760250.953754	44.303437
3501.919287	760251.269627	44.308442
3501.685043	760252.196517	44.313447
3501.828204	760221.830986	44.318452
3501.666580	760213.914609	44.323457
3501.558782	760198.539471	44.328461
3501.694184	760207.348509	44.333466
3501.423581	760212.771057	44.338471
3501.748193	760189.825258	44.343476
3501.563835	760169.677032	44.348481
3501.803401	760167.220055	44.353485
3501.717464	760153.321323	44.358490
3501.568905	760150.089746	44.363495
3501.845415	760125.276888	44.368500
3501.727651	760112.271412	44.373505
3501.602334	760112.341583	44.378509
3501.607288	760112.834263	44.383514
3501.739234	760095.544476	44.388519
3501.309020	760067.641277	44.393524
3501.461304	760067.517561	44.398529
3501.572254	760063.108296	44.403533
3501.559685	760063.061161	44.408538
3501.407326	760063.629178	44.413543
3501.537060	760059.808859	44.418548
3501.128402	760038.414568	44.423553
3501.491309	760026.316271	44.428557
3501.493755	760013.636126	44.433562
3501.460186	760016.355390	44.438567
3501.816878	760016.937966	44.443572
3502.012968	760014.093420	44.448577
3501.635454	759990.226944	44.453581
3501.937400	759965.063991	44.458586
3501.416995	759961.203043	44.463591
3501.854397	759961.574934	44.468596
3501.762798	759963.761083	44.473601
3501.544169	759946.578228	44.478605
3501.721017	759922.619931	44.483610
3501.183344	759931.540515	44.488615
3501.407684	759921.142461	44.493620
3501.714767	759924.101497	44.498625
3501.681097	759912.611278	44.503629
3501.639777	759893.129421	44.508634
3501.306154	759887.954760	44.513639
3501.441162	759874.512393	44.518644
3501.517539	759881.358007	44.523649
3501.302256	759878.038662	44.528653
3501.432474	759870.221714	44.533658
3501.364538	759873.440098	44.538663
3501.489725	759867.696216	44.543668
3501.421448	759853.152607	44.548673
3501.358672	759841.371056	44.553677
3501.576006	759829.839233	44.558682
3501.484866	759828.719616	44.563687
3501.633951	759832.790261	44.568692
3501.511996	759824.176171	44.573697
3501.337145	759824.550565	44.578701
3501.565838	759816.371915	44.583706
3501.700146	759798.439650	44.588711
3501.691943	759780.678911	44.593716
3501.643711	759779.502857	44.598721
3501.173138	759778.149896	44.603725
3501.836277	759779.224588	44.608730
3501.119988	759776.432044	44.613735
3501.538015	759745.772486	44.618740
3501.345858	759738.748773	44.623745
3501.663575	759737.018841	44.628749
3501.422800	759736.417336	44.633754
3501.144855	759734.687156	44.638759
3501.436896	759738.240830	44.643764
3501.534761	759733.093439	44.648769
3501.397018	759736.323416	44.653773
3501.886309	759718.134942	44.658778
3501.775502	759699.157468	44.663783
3501.693098	759685.454654	44.668788
3501.606552	759683.248772	44.673793
3501.699487	759685.897909	44.678797
3501.816893	759659.629616	44.683802
3501.515942	759650.650184	44.688807
3501.499724	759643.399947	44.693812
3501.286876	759635.738131	44.698817
3501.327681	759649.152116	44.703821
3501.420601	759637.788583	44.708826
3501.343255	759639.923130	44.713831
3501.745875	759622.488856	44.718836
3501.463576	759608.424211	44.723841
3501.293954	759608.057640	44.728845
3501.365604	759593.342388	44.733850
3501.336018	759600.797855	44.738855
3501.717622	759587.462254	44.743860
3501.427086	759604.483610	44.748865
3501.681254	759583.817292	44.753869
3501.648492	759571.931680	44.758874
3501.648338	759562.211664	44.763879
3501.564534	759550.630499	44.768884
3501.763639	759552.028612	44.773889
3501.146957	759559.235750	44.778893
3501.900375	759538.092080	44.783898
3501.412852	759527.169687	44.788903
3501.179729	759509.100091	44.793908
3501.418468	759503.978606	44.798913
3501.271428	759511.502912	44.803917
3501.640139	759503.991566	44.808922
3501.304245	759511.399056	44.813927
3501.573227	759507.456768	44.818932
3501.526143	759488.221529	44.823937
3501.475293	759465.878343	44.828941
3501.924589	759457.366803	44.833946
3501.478621	759462.473471	44.838951
3501.381483	759454.446959	44.843956
3501.229463	759466.906298	44.848961
3501.543908	759460.341367	44.853965
3501.800124	759429.065830	44.858970
3501.307330	759425.150698	44.863975
3501.343696	759413.302756	44.868980
3501.526228	759413.371402	44.873985
3501.421736	759415.510497	44.878989
3501.280886	759415.287188	44.883994
3501.373315	759428.495665	44.888999
3501.656444	759424.008236	44.894004
3501.441737	759409.043896	44.899009
3501.330034	759396.973686	44.904013
3501.385313	759375.402169	44.909018
3501.329845	759373.437772	44.914023
3501.186313	759369.119500	44.919028
3501.426171	759370.461571	44.924033
3501.602200	759378.426043	44.929037
3501.215282	759376.319050	44.934042
3501.306958	759376.304026	44.939047
3501.525998	759374.590320	44.944052
3501.522066	759366.350943	44.949057
3501.380303	759344.663873	44.954061
3501.556340	759323.565677	44.959066
3501.698611	759328.821940	44.964071
3501.704643	759320.827580	44.969076
3501.735813	759322.401516	44.974081
3501.473772	759307.346111	44.979085
3501.777460	759285.091834	44.984090
3501.159508	759281.493365	44.989095
3501.586843	759282.755129	44.994100
3501.655982	759274.454235	44.999105
3501.593578	759278.757498	45.004109
3501.616110	759254.575879	45.009114
3501.537520	759240.970317	45.014119
3501.624041	759225.265033	45.019124
3501.286128	759231.488891	45.024129
3501.484627	759229.235773	45.029133
3501.398640	759233.690989	45.034138
3501.254695	759232.283950	45.039143
3501.532304	759226.366366	45.044148
3501.410501	759200.876162	45.049153
3501.191038	759191.487972	45.054157
3501.652904	759185.145160	45.059162
3501.563092	759185.604218	45.064167
3501.374270	759190.175139	45.069172
3501.609017	759183.919202	45.074177
3501.494045	759181.372466	45.079181
3501.671969	759164.270335	45.084186
3501.475706	759149.105059	45.089191
3501.393158	759142.802834	45.094196
3501.808008	759139.477720	45.099201
3501.357752	759140.637811	45.104205
3501.394909	759134.118422	45.109210
3501.636743	759147.154669	45.114215
3501.133668	759112.795963	45.119220
3501.415151	759103.620946	45.124225
3501.553686	759091.360866	45.129229
3501.746956	759098.335904	45.134234
3501.582653	759104.925928	45.139239
3501.701762	759095.333637	45.144244
3501.495135	759095.219875	45.149249
3501.359779	759074.271133	45.154253
3501.712818	759055.906217	45.159258
3501.667466	759060.157442	45.164263
3501.976731	759055.566789	45.169268
3501.487367	759061.470403	45.174273
3501.509922	759034.968901	45.179277
3501.847817	759009.846190	45.184282
3501.615866	759019.704207	45.189287
3501.343800	759010.373829	45.194292
3501.888292	759010.382666	45.199297
3501.743856	758995.356552	45.204301
3501.961795	758973.115532	45.209306
3501.922356	758967.102105	45.214311
3501.531124	758961.738946	45.219316
3501.824869	758935.290972	45.224321
3501.811356	758919.700277	45.229325
3501.977593	758910.840144	45.234330
3501.666618	758917.701293	45.239335
3501.602808	758889.535820	45.244340
3501.859311	758875.775538	45.249345
3501.790957	758874.405286	45.254349
3501.985455	758868.747887	45.259354
3501.499590	758852.050818	45.264359
3501.633965	758842.505032	45.269364
3501.731517	758837.505123	45.274369
3501.485011	758832.858141	45.279373
3501.762231	758819.044988	45.284378
3501.461056	758812.038428	45.289383
3501.576577	758786.014153	45.294388
3501.559305	758776.443998	45.299393
3501.430681	758787.074779	45.304397
3501.803852	758783.904438	45.309402
3501.589611	758779.005361	45.314407
3501.746090	758763.386254	45.319412
3501.767909	758750.404720	45.324417
3501.676847	758748.840812	45.329421
3501.911034	758738.538208	45.334426
3501.504271	758711.662406	45.339431
3501.378418	758692.635553	45.344436
3501.858324	758691.273361	45.349441
3501.432861	758689.468621	45.354445
3501.352284	758687.360155	45.359450
3501.257464	758691.817147	45.364455
3501.499273	758688.569781	45.369460
3501.761603	758689.809569	45.374465
3501.242925	758668.972398	45.379469
3501.218613	758648.201516	45.384474
3501.282874	758647.944287	45.389479
3501.342524	758641.618147	45.394484
3501.549743	758638.228435	45.399489
3501.680879	758646.645219	45.404493
3501.681535	758649.408663	45.409498
3501.501730	758637.052416	45.414503
3501.428764	758611.009343	45.419508
3501.683448	758603.269221	45.424513
3501.724404	758595.564409	45.429517
3501.887474	758586.605728	45.434522
3501.665299	758589.159280	45.439527
3501.465725	758558.448953	45.444532
3501.793250	758549.364357	45.449537
3501.460743	758555.883956	45.454541
3501.558885	758538.892298	45.459546
3501.474358	758546.357879	45.464551
3501.521092	758533.815986	45.469556
3501.627646	758514.848977	45.474561
3501.338279	758509.863444	45.479565
3501.608874	758502.169938	45.484570
3501.588400	758503.653882	45.489575
3501.539241	758511.064306	45.494580
3501.847658	758503.512594	45.499585
3501.673684	758478.077932	45.504589
3501.679235	758457.104201	45.509594
3502.012899	758462.872269	45.514599
3501.448141	758455.711542	45.519604
3501.683456	758431.294747	45.524609
3501.589072	758416.160518	45.529613
3501.701806	758404.150337	45.534618
3501.566103	758408.860993	45.539623
3501.584285	758409.548992	45.544628
3501.457588	758389.189110	45.549633
3501.469749	758379.416196	45.554637
3501.703407	758373.505216	45.559642
3501.537350	758369.042048	45.564647
3501.445286	758373.893561	45.569652
3501.555019	758363.166877	45.574657
3501.388995	758367.142338	45.579661
3501.701701	758355.049686	45.584666
3501.382668	758337.238237	45.589671
3501.481273	758324.440682	45.594676
3501.668759	758318.635988	45.599681
3501.623699	758312.326877	45.604685
3501.776451	758311.166730	45.609690
3501.613551	758290.171026	45.614695
3501.631491	758285.677404	45.619700
3501.638447	758288.686685	45.624705
3501.688429	758287.543517	45.629709
3501.675350	758269.335905	45.634714
3501.232967	758250.409600	45.639719
3501.311846	758235.838574	45.644724
3501.609227	758222.810602	45.649729
3501.676607	758229.905943	45.654733
3501.900670	758221.232851	45.659738
3501.886702	758224.936510	45.664743
3501.695789	758200.688109	45.669748
3501.947461	758181.844340	45.674753
3501.428892	758181.732759	45.679757
3501.944675	758171.382855	45.684762
3501.911465	758160.827558	45.689767
3501.584544	758141.585801	45.694772
3501.780422	758137.753590	45.699777
3501.285393	758139.513426	45.704781
3501.537108	758137.251195	45.709786
3501.359926	758113.740501	45.714791
3501.271654	758108.277318	45.719796
3501.536609	758101.620700	45.724801
3501.443346	758098.823260	45.729805
3501.543185	758095.253651	45.734810
3501.738609	758093.740966	45.739815
3501.559868	758094.461535	45.744820
3501.683290	758049.285413	45.749825
3501.643248	757993.920352	45.754829
3501.724226	757864.211134	45.759834
3501.345868	757690.503395	45.764839
3501.175571	757456.150042	45.769844
3501.403787	757164.717043	45.774849
3500.868044	756839.094974	45.779853
3500.255284	756428.126521	45.784858
3500.051388	755971.159768	45.789863
3499.691693	755460.084807	45.794868
3499.931572	754889.532659	45.799873
3499.417879	754276.254425	45.804877
3499.210658	753584.758385	45.809882
3498.638410	752856.864337	45.814887
3498.299348	752058.977264	45.819892
3498.251198	751200.895656	45.824897
3497.417935	750293.398634	45.829901
3496.592621	749327.197693	45.834906
3496.553264	748305.996852	45.839911
3496.067266	747213.126232	45.844916
3495.275108	746057.034392	45.849921
3494.726502	744864.199017	45.854925
3494.564380	743593.641499	45.859930
3493.457577	742256.028515	45.864935
3492.483093	740874.295988	45.869940
3491.820848	739419.304073	45.874945
3491.205802	737924.801645	45.879949
3490.262784	736354.802188	45.884954
3489.819636	734737.290079	45.889959
3488.941321	733056.252717	45.894964
3487.966598	731315.062116	45.899969
3486.842777	729512.946805	45.904973
3486.072343	727647.010664	45.909978
3485.223319	725729.176080	45.914983
3484.065728	723754.143343	45.919988
3483.044564	721718.974197	45.924993
3481.859056	719630.668716	45.929997
3480.624308	717478.654928	45.935002
3479.375525	715270.620863	45.940007
3477.865026	713016.690836	45.945012
3477.258732	710708.199746	45.950017
3475.831939	708351.052790	45.955021
3474.509603	705920.871542	45.960026
3473.167943	703448.572114	45.965031
3471.989170	700920.425790	45.970036
3470.678793	698337.232898	45.975041
3469.004946	695705.104790	45.980045
3468.041935	693001.640145	45.985050
3466.532857	690260.972583	45.990055
3465.096013	687450.419738	45.995060
3463.429188	684599.498000	46.000065
3461.491910	681698.421031	46.005069
3460.248586	678758.049217	46.010074
3458.877798	675746.293432	46.015079
3457.085472	672685.924009	46.020084
3455.639563	669581.661981	46.025089
3453.868191	666428.096393	46.030093
3452.192684	663206.054660	46.035098
3450.501847	659941.454511	46.040103
3448.575043	656628.356984	46.045108
3447.189369	653272.189696	46.050113
3444.944616	649870.552630	46.055117
3442.922816	646411.784217	46.060122
3441.399720	642906.343041	46.065127
3438.935594	639364.885950	46.070132
3437.660060	635768.371162	46.075137
3435.340577	632124.832681	46.080141
3433.345200	628431.354869	46.085146
3431.124377	624707.476663	46.090151
3429.042415	620933.828256	46.095156
3427.439225	617098.937525	46.100161
3425.102982	613238.960623	46.105165
3423.051169	609320.962840	46.110170
3420.870918	605352.495401	46.115175
3418.748539	601338.260675	46.120180
3416.632850	597281.450840	46.125185
3414.181190	593201.687293	46.130189
3411.722495	589046.700369	46.135194
3409.753763	584884.512312	46.140199
3407.230644	580664.822051	46.145204
3404.834835	576400.154149	46.150209
3402.458952	572099.307146	46.155213
3400.237391	567749.709600	46.160218
3397.635856	563372.873120	46.165223
3394.887276	558956.614971	46.170228
3392.751505	554487.440462	46.175233
3390.268881	549993.705642	46.180237
3387.703221	545453.232197	46.185242
3384.887121	540872.583585	46.190247
3382.508625	536265.456619	46.195252
3380.011792	531608.374429	46.200257
3377.160398	526918.318007	46.205261
3374.678508	522183.346248	46.210266
3371.668454	517435.974753	46.215271
3368.978650	512643.991775	46.220276
3366.265222	507806.582825	46.225281
3363.245981	502947.193546	46.230285
3360.280107	498044.228699	46.235290
3357.872864	493122.083702	46.240295
3354.877235	488158.037661	46.245300
3352.059960	483175.953941	46.250305
3348.849012	478150.322569	46.255309
3345.965678	473097.684345	46.260314
3343.063770	468013.041491	46.265319
3339.880134	462912.763213	46.270324
3337.489190	457766.939363	46.275329
3334.153664	452583.665025	46.280333
3331.126851	447391.545604	46.285338
3328.155212	442156.056993	46.290343
3324.704593	436912.809247	46.295348
3321.734679	431621.937818	46.300353
3318.537595	426325.239228	46.305357
3315.168740	420993.696396	46.310362
3312.186023	415636.246483	46.315367
3309.155602	410264.107202	46.320372
3305.860717	404850.367890	46.325377
3302.614833	399425.606393	46.330381
3299.201348	393973.425733	46.335386
3295.704980	388502.605512	46.340391
3292.277985	383022.480522	46.345396
3289.128163	377509.484391	46.350401
3285.201788	371991.050341	46.355405
3281.671321	366439.455301	46.360410
3278.803526	360888.562876	46.365415
3274.879560	355312.039781	46.370420
3271.402711	349719.617738	46.375425
3267.807265	344116.821787	46.380429
3264.162961	338489.327103	46.385434
3260.526991	332845.227661	46.390439
3257.150305	327209.592684	46.395444
3253.330609	321558.707186	46.400449
3249.706287	315891.207377	46.405453
3246.265545	310211.260246	46.410458
3242.698106	304517.966211	46.415463
3238.584548	298826.307654	46.420468
3234.876643	293114.476828	46.425473
3231.029436	287405.525430	46.430477
3227.311976	281679.590926	46.435482
3223.408194	275954.087439	46.440487
3219.749232	270225.169421	46.445492
3215.768152	264495.166655	46.450497
3211.938943	258750.930539	46.455501
3208.121270	253012.115451	46.460506
3204.084382	247263.932448	46.465511
3200.125449	241523.696954	46.470516
3196.446163	235767.380845	46.475521
3192.240065	230015.410748	46.480525
3188.167393	224266.399393	46.485530
3184.148361	218514.829609	46.490535
3180.052982	212766.371452	46.495540
3175.968644	206950.112129	46.500545
3171.517215	201212.241873	46.505549
3167.690992	195475.875364	46.510554
3163.282710	189754.303134	46.515559
3159.171123	184036.745067	46.520564
3155.257914	178327.232066	46.525569
3151.013230	172627.090864	46.530573
3146.605391	166941.335370	46.535578
3142.332466	161258.000027	46.540583
3137.724440	155599.717132	46.545588
3133.676592	149924.766942	46.550593
3128.922012	144295.480314	46.555597
3124.486302	138672.749224	46.560602
3120.081698	133065.012383	46.565607
3115.286368	127481.220122	46.570612
3110.540855	121902.475998	46.575617
3105.954556	116357.726284	46.580621
3101.271020	110826.754464	46.585626
3096.681198	105324.000230	46.590631
3091.749875	99858.662306	46.595636
3087.367551	94400.746257	46.600641
3082.148766	88987.760353	46.605645
3077.377950	83593.057375	46.610650
3072.577534	78228.145743	46.615655
3067.635139	72899.529105	46.620660
3062.661644	67595.848837	46.625665
3057.144193	62339.705689	46.630669
3051.843814	57106.678707	46.635674
3046.737897	51930.815183	46.640679
3041.265736	46796.650182	46.645684
3036.006629	41702.832797	46.650689
3030.305440	36651.010509	46.655693
3024.603805	31646.793616	46.660698
3018.467182	26698.459730	46.665703
3012.497520	21839.858958	46.670708
3006.566131	17009.671682	46.675713
2999.141615	12285.369521	46.680717
2988.011969	7736.993432	46.685722
2971.026183	3470.798817	46.690727
2917.480498	401.512152	46.695732
2777.933135	247.676691	46.700737
2686.004733	255.559760	46.705741
2657.604121	248.326139	46.710746
2675.869517	224.487785	46.715751
2715.405931	218.273084	46.720756
2755.153422	214.434894	46.725761
2783.115063	219.549610	46.730765
2796.415589	226.293472	46.735770
2798.850330	212.038584	46.740775
2794.341676	218.635274	46.745780
2787.816310	203.174489	46.750785
2780.847477	219.969173	46.755789
2775.764904	221.143077	46.760794
2771.845494	225.504288	46.765799
2768.981216	227.714898	46.770804
2767.430087	209.048918	46.775809
2765.628282	218.048355	46.780813
2762.723398	214.541475	46.785818
2760.145438	204.306479	46.790823
2757.059794	217.280099	46.795828
2754.262173	208.510988	46.800833
2751.173278	207.417641	46.805837
2748.239228	204.247131	46.810842
2745.042187	198.676903	46.815847
2741.058215	210.440940	46.820852
2737.816822	207.311640	46.825857
2734.711618	210.415839	46.830861
2731.874743	207.625511	46.835866
2728.503220	199.299134	46.840871
2725.386488	198.536023	46.845876
2722.190417	196.213259	46.850881
2718.596423	203.868693	46.855885
2715.610068	205.642112	46.860890
2712.445070	191.750751	46.865895
2708.843345	199.158824	46.870900
2705.470120	202.703467	46.875905
2702.357340	197.822839	46.880909
2698.628352	191.070635	46.885914
2695.350917	195.336488	46.890919
2691.631815	194.970113	46.895924
2688.821308	192.029619	46.900929
2685.538746	196.052220	46.905933
2681.682941	190.988340	46.910938
2678.678044	190.123475	46.915943
2675.131441	193.518446	46.920948
2671.440369	183.784327	46.925953
2668.647882	185.277233	46.930957
2665.208861	182.858964	46.935962
2661.824113	189.882255	46.940967
2658.108881	193.968806	46.945972
2654.086392	183.132572	46.950977
2651.033418	192.888550	46.955981
2648.272761	188.829803	46.960986
2644.836619	181.149243	46.965991
2641.285298	191.599082	46.970996
2637.860207	183.655026	46.976001
2633.863463	183.245469	46.981005
2630.108924	182.892513	46.986010
2626.669097	180.405343	46.991015
2623.866028	175.027130	46.996020
2620.413690	177.974365	47.001025
2616.693724	178.713491	47.006029
2613.652985	186.398371	47.011034
2610.352796	178.101741	47.016039
2606.672590	192.384532	47.021044
2602.999502	187.159446	47.026049
2599.943532	175.558417	47.031053
2596.333722	178.761050	47.036058
2593.056649	180.051249	47.041063
2589.151738	186.948571	47.046068
2585.930049	176.530998	47.051073
2582.144723	179.955105	47.056077
2578.744086	183.082864	47.061082
2575.573654	180.086599	47.066087
2571.468304	177.248681	47.071092
2568.383717	184.507493	47.076097
2565.421000	173.409463	47.081101
2561.728040	182.336857	47.086106
2558.498508	171.066136	47.091111
2554.585420	180.742372	47.096116
2551.574013	177.490490	47.101121
2547.854736	182.721768	47.106125
2544.404609	176.239484	47.111130
2540.918434	170.529636	47.116135
2536.873697	178.477097	47.121140
2533.433604	180.745701	47.126145
2530.421691	179.095909	47.131149
2526.827027	175.049835	47.136154
2523.850489	174.626764	47.141159
2519.609253	177.409485	47.146164
2516.237295	172.154160	47.151169
2513.164900	177.935490	47.156173
2509.221604	178.118687	47.161178
2506.230328	170.404851	47.166183
2502.742345	177.899617	47.171188
2498.985074	172.921430	47.176193
2495.551482	169.788833	47.181197
2491.929495	175.032264	47.186202
2488.466405	160.433503	47.191207
2485.033767	175.012623	47.196212
2481.928999	168.188255	47.201217
2478.483654	164.794371	47.206221
2474.334030	163.421816	47.211226
2471.252241	168.037276	47.216231
2467.462361	164.600994	47.221236
2463.947794	169.582157	47.226241
2460.855352	159.182968	47.231245
2457.323000	166.282738	47.236250
2454.143903	164.779288	47.241255
2450.253753	169.046131	47.246260
2446.868179	165.501871	47.251265
2443.263520	167.443180	47.256269
2439.605099	171.374271	47.261274
2436.384140	162.923386	47.266279
2432.615253	165.577056	47.271284
2429.222588	162.411888	47.276289
2425.983843	164.020881	47.281293
2422.321540	162.687659	47.286298
2418.753451	157.527261	47.291303
2415.249100	165.405856	47.296308
2412.030383	166.979771	47.301313
2408.656130	159.387064	47.306317
2404.769232	160.802470	47.311322
2401.436784	153.518589	47.316327
2397.677464	159.411578	47.321332
2394.391613	147.028088	47.326337
2390.870270	146.056360	47.331341
2387.085188	159.904153	47.336346
2384.097446	150.434127	47.341351
2380.327014	157.020441	47.346356
2377.104920	157.499323	47.351361
2373.653476	161.973599	47.356365
2369.978379	170.731428	47.361370
2366.534868	156.506462	47.366375
2362.495109	163.075434	47.371380
2359.314725	158.108997	47.376385
2356.031152	146.613579	47.381389
2352.265197	160.217282	47.386394
2349.134028	145.188957	47.391399
2345.760331	166.225538	47.396404
2342.292437	151.999310	47.401409
2338.309969	162.724805	47.406413
2334.691208	165.045849	47.411418
2331.337471	159.791813	47.416423
2328.182452	157.890588	47.421428
2324.954683	156.113502	47.426433
2321.760893	160.898970	47.431437
2317.726555	155.944946	47.436442
2314.007260	149.444707	47.441447
2310.606605	162.494005	47.446452
2307.124551	161.330341	47.451457
2303.742584	163.968977	47.456461
2299.854308	162.562585	47.461466
2296.200570	153.528347	47.466471
2292.946505	155.466373	47.471476
2289.600224	155.380984	47.476481
2286.167894	151.255358	47.481485
2282.518968	150.422072	47.486490
2279.090498	150.191251	47.491495
2275.445036	156.733864	47.496500
2271.962599	153.507133	47.501505
2268.616731	149.565328	47.506509
2265.223536	150.579991	47.511514
2261.928030	153.732806	47.516519
2258.330615	155.957234	47.521524
2254.624545	154.222528	47.526529
2251.489712	144.122806	47.531533
2247.522181	162.639929	47.536538
2244.467782	141.393124	47.541543
2240.619401	146.144005	47.546548
2236.893780	147.114100	47.551553
2233.517281	143.883275	47.556557
2230.193023	148.715281	47.561562
2226.836302	146.790912	47.566567
2222.930268	143.351018	47.571572
2219.184266	145.620812	47.576577
2216.561792	145.240348	47.581581
2212.805747	154.511950	47.586586
2209.136153	146.182356	47.591591
2205.712579	152.504151	47.596596
2202.256631	150.653861	47.601601
2198.878521	142.690994	47.606605
2195.182781	147.635279	47.611610
2191.588127	157.573606	47.616615
2188.093749	153.315472	47.621620
2184.447879	155.130818	47.626625
2181.178350	146.352736	47.631629
2177.652060	148.748972	47.636634
2174.255412	135.562337	47.641639
2170.463470	146.118460	47.646644
2167.143198	141.849661	47.651649
2163.831048	139.915001	47.656653
2159.868490	146.491487	47.661658
2156.726927	133.979932	47.666663
2153.407517	136.902745	47.671668
2149.638987	150.010520	47.676673
2146.453077	139.409040	47.681677
2142.637431	143.338990	47.686682
2139.372470	136.719256	47.691687
2135.427230	150.294010	47.696692
2131.795679	149.762272	47.701697
2128.857817	131.257819	47.706701
2125.219925	142.830787	47.711706
2122.005332	133.536704	47.716711
2118.017447	151.678004	47.721716
2114.728048	143.694200	47.726721
2111.378226	148.278531	47.731725
2107.578714	148.129848	47.736730
2104.023564	139.588799	47.741735
2100.686426	137.934997	47.746740
2097.199692	137.600117	47.751745
2093.900090	143.072640	47.756749
2090.248731	146.355978	47.761754
2086.851563	134.169815	47.766759
2083.180024	146.264230	47.771764
2079.588144	137.592734	47.776769
2076.220207	138.957978	47.781773
2072.540236	134.296167	47.786778
2069.332236	129.489857	47.791783
2065.830990	131.923475	47.796788
2061.929161	134.546211	47.801793
2058.468850	134.786958	47.806797
2054.690599	144.625165	47.811802
2051.745392	128.591474	47.816807
2047.888078	134.171235	47.821812
2044.924249	134.260269	47.826817
2041.756362	137.619830	47.831821
2037.918247	132.560771	47.836826
2034.323912	138.576895	47.841831
2030.767197	145.732526	47.846836
2026.909560	137.603785	47.851841
2023.505855	134.851850	47.856845
2020.017328	139.725635	47.861850
2016.670737	127.740539	47.866855
2013.067788	136.471876	47.871860
2009.591611	134.864080	47.876865
2006.048630	129.463895	47.881869
2002.398532	135.154403	47.886874
1999.252264	129.669346	47.891879
1995.734334	136.471658	47.896884
1992.173231	127.541180	47.901889
1989.039005	132.066589	47.906893
1985.438654	139.727364	47.911898
1981.783080	129.129665	47.916903
1978.156915	130.819574	47.921908
1974.513296	140.913187	47.926913
1971.317060	129.258423	47.931917
1967.560369	140.993869	47.936922
1964.133179	132.493717	47.941927
1960.576257	131.780451	47.946932
1957.060460	133.696392	47.951937
1953.847732	127.587359	47.956941
1949.803465	137.159516	47.961946
1946.690922	132.645334	47.966951
1942.582423	134.966167	47.971956
1939.519653	130.772899	47.976961
1936.329017	125.185925	47.981965
1932.788669	126.191893	47.986970
1929.513938	125.982063	47.991975
1925.487414	124.712807	47.996980
1922.102378	137.254975	48.001985
1918.400321	127.836037	48.006989
1914.897237	135.817403	48.011994
1911.635429	135.514869	48.016999
1908.416984	129.386495	48.022004
1904.427385	132.950021	48.027009
1901.130958	133.459350	48.032013
1897.565211	131.219825	48.037018
1894.171442	129.785350	48.042023
1890.768680	138.127219	48.047028
1887.091024	132.885427	48.052033
1883.825158	127.723001	48.057037
1880.145960	134.462934	48.062042
1876.761525	129.360421	48.067047
1873.062629	134.604659	48.072052
1869.346077	132.313980	48.077057
1866.676552	123.839908	48.082061
1862.214704	135.988110	48.087066
1858.650502	130.174212	48.092071
1856.012436	137.637321	48.097076
1852.388603	129.843177	48.102081
1848.933707	130.236139	48.107085
1844.655487	137.261866	48.112090
1841.382231	129.780028	48.117095
1838.023021	127.596508	48.122100
1834.487496	131.156276	48.127105
1831.827842	130.202844	48.132109
1828.115500	132.062273	48.137114
1824.292117	132.266108	48.142119
1820.621734	124.312768	48.147124
1816.509322	128.998457	48.152129
1813.213963	119.810200	48.157133
1809.403356	124.907440	48.162138
1806.754466	126.590425	48.167143
1803.230005	122.305664	48.172148
1799.640330	125.029048	48.177153
1796.254365	119.978170	48.182157
1792.344252	123.878699	48.187162
1788.995075	121.514575	48.192167
1785.502178	128.162924	48.197172
1782.198856	127.533680	48.202177
1778.907640	116.801208	48.207181
1774.967216	128.715650	48.212186
1771.637499	117.917144	48.217191
1768.252181	120.559320	48.222196
1764.520495	132.253677	48.227201
1760.956828	126.141807	48.232205
1757.559287	127.018087	48.237210
1754.279616	122.331275	48.242215
1750.597600	127.065270	48.247220
1746.909229	116.640792	48.252225
1743.399769	126.359897	48.257229
1739.873693	127.306438	48.262234
1736.379963	117.488876	48.267239
1732.859978	123.403325	48.272244
1729.455042	124.484505	48.277249
1726.069044	122.086677	48.282253
1722.565884	122.000328	48.287258
1719.043145	121.081709	48.292263
1715.469254	122.499738	48.297268
1711.904450	108.885213	48.302273
1708.398788	120.663697	48.307277
1705.102095	115.173832	48.312282
1701.801619	117.523162	48.317287
1698.096238	120.506168	48.322292
1694.587150	129.494123	48.327297
1691.040533	111.316963	48.332301
1686.994957	115.403635	48.337306
1683.984976	114.896737	48.342311
1680.630065	128.998154	48.347316
1676.960554	114.119718	48.352321
1673.798172	105.513596	48.357325
1670.003426	124.591126	48.362330
1666.312725	118.769180	48.367335
1662.928069	117.855543	48.372340
1659.314321	123.659104	48.377345
1656.321550	115.022505	48.382349
1652.730666	119.915326	48.387354
1648.627977	115.187255	48.392359
1645.464095	114.762140	48.397364
1641.945582	120.749630	48.402369
1638.797747	107.793628	48.407373
1634.708372	120.444074	48.412378
1631.422489	111.003999	48.417383
1628.396544	116.739534	48.422388
1624.455380	120.725878	48.427393
1621.172758	109.245811	48.432397
1617.385718	124.737507	48.437402
1613.533696	113.776711	48.442407
1610.403257	115.828164	48.447412
1606.912442	107.995446	48.452417
1603.626250	106.235543	48.457421
1599.630908	120.605402	48.462426
1596.238373	113.170405	48.467431
1593.018509	113.338530	48.472436
1589.271502	118.014765	48.477441
1586.102541	105.988608	48.482445
1582.302816	109.740784	48.487450
1579.167650	108.091430	48.492455
1575.658744	111.946355	48.497460
1571.942848	115.591303	48.502465
1568.733277	122.332559	48.507469
1564.792158	122.660947	48.512474
1560.900322	118.417196	48.517479
1557.796364	113.507836	48.522484
1554.163434	118.886053	48.527489
1551.290918	112.061862	48.532493
1546.734370	112.299320	48.537498
1543.957953	110.166040	48.542503
1540.400906	113.848613	48.547508
1536.963162	114.090799	48.552513
1533.609056	108.536016	48.557517
1529.850241	119.356121	48.562522
1526.484771	117.284219	48.567527
1523.022753	111.573880	48.572532
1518.976515	117.757313	48.577537
1515.659156	113.130438	48.582541
1511.997887	117.346349	48.587546
1508.888150	115.663826	48.592551
1505.421395	121.993311	48.597556
1501.862999	114.171502	48.602561
1498.434996	110.473100	48.607565
1494.553275	118.724777	48.612570
1491.450655	110.581915	48.617575
1488.147778	117.072890	48.622580
1484.111678	114.598966	48.627585
1481.033680	111.698775	48.632589
1477.613401	124.519018	48.637594
1474.016881	122.794108	48.642599
1469.919900	119.475043	48.647604
1466.895914	124.325912	48.652609
1463.702160	103.367267	48.657613
1459.667569	117.796439	48.662618
1455.993362	105.736579	48.667623
1452.867971	106.937590	48.672628
1449.337620	110.293565	48.677633
1445.666522	99.480362	48.682637
1442.114248	114.368283	48.687642
1438.539116	113.516027	48.692647
1435.147803	117.323153	48.697652
1431.638146	109.092743	48.702657
1428.396689	114.431993	48.707661
1425.034476	117.748068	48.712666
1421.580432	116.763463	48.717671
1417.821220	105.239100	48.722676
1414.261286	118.075638	48.727681
1410.751013	107.454441	48.732685
1407.167130	117.830047	48.737690
1403.625443	106.075840	48.742695
1400.482066	105.401445	48.747700
1396.598799	114.609747	48.752705
1393.288739	103.795523	48.757709
1389.446600	109.197130	48.762714
1385.909655	115.659317	48.767719
1382.787971	110.918213	48.772724
1379.232041	110.771259	48.777729
1375.979315	101.139842	48.782733
1372.495991	111.747041	48.787738
1369.074439	109.582359	48.792743
1365.270158	109.509958	48.797748
1361.245404	110.768645	48.802753
1358.079602	110.917732	48.807757
1354.544610	110.289382	48.812762
1351.376628	108.609543	48.817767
1347.860620	117.398813	48.822772
1343.962093	104.058083	48.827777
1340.723388	105.294354	48.832781
1337.094126	107.611288	48.837786
1333.284235	107.334029	48.842791
1330.257250	99.214486	48.847796
1327.059965	105.011997	48.852801
1323.109176	108.064657	48.857805
1319.577687	106.554265	48.862810
1316.065837	109.507485	48.867815
1312.945155	102.521398	48.872820
1309.176667	112.054297	48.877825
1305.880579	100.306028	48.882829
1301.975760	108.187161	48.887834
1298.292606	110.892543	48.892839
1294.980413	107.602544	48.897844
1291.449050	109.560311	48.902849
1287.995682	108.963673	48.907853
1285.041014	108.834679	48.912858
1281.449299	108.662768	48.917863
1278.080977	111.095325	48.922868
1274.169350	108.172561	48.927873
1270.657622	108.111318	48.932877
1266.993790	112.440744	48.937882
1263.427727	119.234453	48.942887
1260.005409	110.858494	48.947892
1256.438096	116.541224	48.952897
1253.205146	111.220763	48.957901
1249.712155	106.558339	48.962906
1246.349070	105.504534	48.967911
1242.857363	101.914616	48.972916
1239.012535	108.564552	48.977921
1235.852878	106.545195	48.982925
1231.830463	110.690036	48.987930
1228.450626	110.923278	48.992935
1225.413488	97.486756	48.997940
1221.304236	107.314243	49.002945
1218.102330	98.784352	49.007949
1214.193561	99.880483	49.012954
1210.971706	101.026843	49.017959
1207.861562	111.660665	49.022964
1204.005134	107.201645	49.027969
1200.508739	99.592646	49.032973
1196.928513	102.042466	49.037978
1193.750746	105.361675	49.042983
1190.538433	102.017113	49.047988
1186.557803	105.986936	49.052993
1183.166735	100.502346	49.057997
1179.890233	103.699220	49.063002
1176.259663	93.502368	49.068007
1172.648306	94.662665	49.073012
1168.830721	101.401285	49.078017
1165.378756	91.110088	49.083021
1161.753276	91.577135	49.088026
1158.428275	101.336328	49.093031
1155.014914	99.497464	49.098036
1151.449669	104.109004	49.103041
1148.381010	101.047302	49.108045
1144.301477	100.370173	49.113050
1140.793607	95.777024	49.118055
1137.831314	99.332648	49.123060
1133.987632	93.058485	49.128065
1130.461171	104.082294	49.133069
1126.562486	107.610759	49.138074
1123.539627	97.369961	49.143079
1119.964741	104.206491	49.148084
1116.287408	100.665250	49.153089
1112.890725	106.530738	49.158093
1109.517437	104.047875	49.163098
1105.891737	97.819268	49.168103
1102.417364	101.885732	49.173108
1098.998461	96.417681	49.178113
1095.518604	98.070087	49.183117
1091.992577	99.390939	49.188122
1088.530177	100.674795	49.193127
1084.837893	96.030602	49.198132
1081.488302	101.279525	49.203137
1078.199477	102.935176	49.208141
1074.451768	101.446483	49.213146
1070.882750	103.063188	49.218151
1067.670219	98.765053	49.223156
1063.872380	105.682238	49.228161
1060.545670	101.046275	49.233165
1056.861018	107.013465	49.238170
1053.379183	97.413266	49.243175
1049.932481	103.452667	49.248180
1046.343612	89.303144	49.253185
1042.623608	86.304230	49.258189
1039.314631	97.016736	49.263194
1035.840432	104.808498	49.268199
1032.579270	103.993712	49.273204
1029.407309	107.880211	49.278209
1026.020197	90.363862	49.283213
1022.211574	96.342772	49.288218
1018.099628	107.099158	49.293223
1014.706409	97.399833	49.298228
1011.275593	98.823358	49.303233
1007.923009	97.147011	49.308237
1004.110541	100.225770	49.313242
1000.776096	104.119521	49.318247
997.380728	97.379987	49.323252
993.988284	96.265366	49.328257
990.481253	95.728615	49.333261
986.755883	96.863208	49.338266
983.320860	101.953919	49.343271
979.988544	102.494830	49.348276
976.425444	100.768198	49.353281
973.059163	95.154583	49.358285
969.066814	94.579994	49.363290
965.681459	98.166685	49.368295
962.314822	100.310132	49.373300
958.836349	101.136587	49.378305
955.310237	93.155659	49.383309
951.722774	99.394918	49.388314
948.116999	98.324229	49.393319
945.097453	93.083283	49.398324
941.249396	91.292091	49.403329
937.924556	91.025097	49.408333
934.312158	93.353804	49.413338
931.149449	93.609481	49.418343
927.364633	93.436599	49.423348
923.596031	94.508177	49.428353
920.219016	92.726246	49.433357
916.982069	90.094439	49.438362
913.122537	87.839474	49.443367
910.060075	88.654547	49.448372
906.300167	88.996144	49.453377
902.787934	84.382638	49.458381
899.231738	81.791799	49.463386
895.363362	92.085177	49.468391
892.128497	86.673210	49.473396
888.458755	92.399100	49.478401
885.211723	87.638781	49.483405
881.846893	90.182188	49.488410
878.330069	94.070592	49.493415
875.115039	82.195837	49.498420
871.284900	102.287801	49.503425
867.799912	82.655095	49.508429
864.278222	89.689418	49.513434
860.808083	94.795924	49.518439
857.418834	83.690103	49.523444
853.662629	92.651251	49.528449
850.271938	93.570780	49.533453
846.581896	89.816628	49.538458
843.260691	89.651332	49.543463
839.746527	88.435498	49.548468
836.251010	92.452221	49.553473
832.813159	90.238045	49.558477
829.285699	92.957874	49.563482
825.453010	97.408076	49.568487
822.052426	88.150618	49.573492
818.210341	96.806770	49.578497
815.340566	85.607062	49.583501
812.037285	93.358988	49.588506
808.318251	95.768856	49.593511
804.944486	82.642587	49.598516
800.962161	95.942988	49.603521
797.696728	90.399822	49.608525
794.123499	88.297153	49.613530
790.168217	91.318128	49.618535
787.474702	88.087892	49.623540
783.768504	91.893166	49.628545
780.645901	92.771605	49.633549
776.894682	89.774586	49.638554
773.028402	98.896360	49.643559
769.746055	84.643963	49.648564
765.947367	88.318186	49.653569
762.669074	94.271454	49.658573
759.064460	96.859115	49.663578
755.170329	93.119795	49.668583
752.099342	83.453281	49.673588
748.950250	98.059286	49.678593
745.140473	89.068749	49.683597
741.989330	94.622637	49.688602
738.122810	91.164885	49.693607
734.492993	85.396733	49.698612
730.917056	97.861512	49.703617
727.564243	85.414023	49.708621
723.991675	90.741890	49.713626
720.183951	92.459719	49.718631
716.771924	93.231552	49.723636
713.440314	98.623421	49.728641
710.423531	86.040239	49.733645
706.529329	85.981246	49.738650
703.090840	94.702708	49.743655
699.788482	93.850846	49.748660
696.175903	87.710463	49.753665
692.740464	94.685424	49.758669
689.277772	85.814133	49.763674
685.906259	90.574472	49.768679
682.362683	83.573721	49.773684
678.645041	86.461816	49.778689
675.087218	90.692080	49.783693
671.456869	93.496622	49.788698
667.668526	86.509095	49.793703
664.549628	84.607776	49.798708
660.776408	89.242238	49.803713
657.425803	87.046299	49.808717
654.139657	96.771598	49.813722
650.467862	97.313909	49.818727
646.777423	83.903141	49.823732
643.309051	80.060887	49.828737
639.993905	78.669327	49.833741
636.706639	84.980171	49.838746
633.358970	94.268148	49.843751
630.072364	78.452743	49.848756
625.727633	85.128231	49.853761
622.532270	84.828174	49.858765
619.405264	82.338610	49.863770
615.319653	93.957292	49.868775
611.957669	86.133179	49.873780
608.208550	93.966204	49.878785
604.932742	90.079774	49.883789
601.405946	90.772101	49.888794
597.687951	83.042445	49.893799
594.692275	92.333766	49.898804
591.050128	87.681159	49.903809
587.810487	87.495044	49.908813
584.182652	85.413487	49.913818
580.631248	91.825468	49.918823
577.334343	82.240044	49.923828
573.189255	85.974147	49.928833
569.632459	81.188794	49.933837
566.328297	89.326251	49.938842
563.151501	80.501742	49.943847
559.468159	74.225257	49.948852
555.520809	83.729303	49.953857
552.512689	75.170822	49.958861
549.136928	78.379957	49.963866
545.442486	88.893403	49.968871
542.160338	84.721163	49.973876
538.586526	87.143677	49.978881
535.072470	73.628371	49.983885
531.434161	86.371046	49.988890
527.788711	92.588730	49.993895
524.334923	89.969010	49.998900
520.822656	85.236496	50.003905
517.316927	86.243898	50.008909
514.103649	80.243997	50.013914
510.453123	84.936367	50.018919
506.717452	85.175075	50.023924
502.964220	83.953482	50.028929
499.714338	91.538524	50.033933
496.751251	83.171914	50.038938
492.790500	82.158845	50.043943
489.749130	77.913907	50.048948
485.887626	89.001171	50.053953
482.464053	84.953705	50.058957
479.000510	74.469781	50.063962
475.260671	89.101658	50.068967
471.952159	81.102058	50.073972
468.087172	88.782182	50.078977
464.618413	87.440761	50.083981
461.592652	82.398398	50.088986
457.834571	92.896643	50.093991
454.437656	79.726436	50.098996
450.654251	94.566262	50.104001
447.386189	80.594801	50.109005
443.553996	83.773873	50.114010
440.220226	89.191779	50.119015
437.438104	75.400888	50.124020
433.322786	93.395751	50.129025
430.016168	84.390466	50.134029
426.394492	83.451189	50.139034
422.652384	84.519648	50.144039
419.628106	85.713964	50.149044
415.661468	86.547407	50.154049
412.016496	88.867998	50.159053
408.979801	76.663938	50.164058
405.005706	90.128889	50.169063
401.602076	82.796353	50.174068
398.051524	89.769566	50.179073
394.892360	84.230041	50.184077
391.611944	88.027906	50.189082
387.995174	90.646345	50.194087
384.506439	77.206913	50.199092
380.741171	92.343334	50.204097
377.181020	79.943676	50.209101
373.692226	82.132391	50.214106
370.162700	82.928791	50.219111
366.924867	80.696824	50.224116
363.269641	91.000072	50.229121
359.614894	76.211458	50.234125
356.350046	80.807341	50.239130
352.566525	86.289179	50.244135
349.252843	83.789813	50.249140
345.937782	93.238163	50.254145
342.571938	93.479730	50.259149
338.780920	77.018495	50.264154
334.870037	87.411794	50.269159
331.904431	87.977796	50.274164
328.227741	86.492263	50.279169
324.581215	89.343822	50.284173
321.216800	82.295917	50.289178
317.710405	101.361296	50.294183
314.234711	78.337906	50.299188
310.665873	86.480662	50.304193
307.300508	84.487000	50.309197
303.744063	88.309879	50.314202
299.625945	92.518523	50.319207
296.585346	87.817784	50.324212
293.026603	73.544517	50.329217
289.564299	86.505213	50.334221
286.817024	84.739413	50.339226
282.904360	86.993306	50.344231
279.505828	76.738743	50.349236
275.392562	85.998700	50.354241
271.919358	86.105631	50.359245
268.773124	83.539842	50.364250
264.984796	87.403453	50.369255
261.504073	84.668482	50.374260
258.431755	80.276545	50.379265
254.294379	82.055331	50.384269
251.178131	83.327222	50.389274
247.308033	94.132373	50.394279
244.484470	72.252204	50.399284
240.839633	84.208063	50.404289
237.239959	88.141982	50.409293
233.802535	81.426761	50.414298
229.850639	90.277328	50.419303
226.592439	82.957507	50.424308
222.930009	84.571770	50.429313
219.895607	86.146214	50.434317
216.520948	85.920302	50.439322
212.495577	93.338033	50.444327
209.134497	79.315578	50.449332
205.126835	79.351933	50.454337
201.751491	81.406516	50.459341
198.842772	74.429042	50.464346
195.164631	82.845209	50.469351
192.087450	80.283406	50.474356
187.900311	85.082608	50.479361
184.862367	87.215526	50.484365
181.422795	78.327499	50.489370
177.576123	92.643301	50.494375
173.972037	84.187344	50.499380
170.121658	83.914036	50.504385
166.640843	82.340669	50.509389
163.680618	78.227174	50.514394
160.133319	83.279620	50.519399
156.896155	77.923377	50.524404
153.138262	83.557434	50.529409
149.396565	74.049116	50.534413
146.112610	70.852760	50.539418
142.362497	84.559954	50.544423
139.302336	80.353764	50.549428
135.344302	83.926816	50.554433
131.806858	86.131733	50.559437
128.745732	82.079236	50.564442
125.157526	76.704993	50.569447
121.989408	83.126299	50.574452
117.985346	78.108289	50.579457
114.245109	84.502531	50.584461
111.015292	76.693855	50.589466
107.530374	79.979928	50.594471
104.007951	78.519503	50.599476
100.582020	75.739079	50.604481
96.802009	80.345216	50.609485
93.720235	79.775732	50.614490
89.656794	84.572046	50.619495
86.626557	71.620719	50.624500
83.023130	77.560293	50.629505
79.479597	87.131477	50.634509
76.195646	76.716003	50.639514
72.304547	89.103259	50.644519
69.065408	80.975112	50.649524
65.260930	85.377163	50.654529
61.552457	80.233722	50.659533
58.658431	86.272287	50.664538
54.753860	81.981160	50.669543
51.591715	76.554335	50.674548
48.091534	85.970737	50.679553
44.851238	80.939531	50.684557
41.355902	79.073096	50.689562
37.308839	83.640206	50.694567
33.783223	76.136906	50.699572
29.922860	84.000199	50.704577
26.909492	78.102108	50.709581
23.667897	84.920107	50.714586
20.058958	82.076445	50.719591
16.521102	86.000494	50.724596
12.627149	78.598889	50.729601
8.973446	80.058191	50.734605
5.952317	79.140475	50.739610
2.600701	76.004437	50.744615