Number of Data Points = 25
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3866_Position 104_00000.hld	3384.215351	1058230.816530	6730.114539	278833572.676326	3522.624978	3502.143970	357.095808	3.795206	0.309547	3106.578067	2.515712	-133.123000	-61.040000	0.028151
3866_Position 104_00001.hld	3382.605838	988877.444043	6254.148438	278568042.779426	3521.293335	3501.192419	331.999452	3.549860	0.146820	3088.428089	2.610525	-133.074000	-61.040000	-0.223064
3866_Position 104_00002.hld	3389.337824	978047.177991	6611.623380	279679497.871186	3520.614441	3500.284160	350.277805	3.497029	0.032201	3078.613926	2.850501	-133.024000	-61.040000	-0.318671
3866_Position 104_00003.hld	3366.865235	1086588.446889	5998.814528	275977916.366716	3521.599053	3502.715632	319.935990	3.937230	0.490587	3067.190181	2.404440	-132.974000	-61.040000	-0.301568
3866_Position 104_00004.hld	3365.411412	1037719.503201	5696.770502	275739300.662066	3521.758464	3502.030858	303.958447	3.763408	1.960086	3101.431502	2.199171	-132.924000	-61.040000	-0.316638
3866_Position 104_00005.hld	3380.138110	1047267.872683	6464.366464	278161174.947642	3521.270827	3501.642809	343.409686	3.764968	0.448369	3104.641321	2.450532	-133.124000	-60.990000	-0.218185
3866_Position 104_00006.hld	3382.311231	1029246.390098	6445.507545	278519453.679397	3521.343128	3502.074459	342.187533	3.695420	0.116693	3079.681779	2.645173	-133.074000	-60.990000	-0.255625
3866_Position 104_00007.hld	3375.055838	1105098.590629	6486.131304	277324172.083897	3521.607587	3502.839860	345.085493	3.984862	0.291522	3076.596067	2.501743	-133.024000	-60.990000	-0.170666
3866_Position 104_00008.hld	3364.799515	1092113.175609	5951.606645	275638900.962422	3522.061170	3502.423678	317.613383	3.962116	0.846468	3076.041718	2.323622	-132.974000	-60.990000	-0.167335
3866_Position 104_00009.hld	3366.909313	1088994.770097	6000.177569	275985152.545451	3523.027559	3503.029631	320.004490	3.945845	0.855143	3080.985448	2.325392	-132.924000	-60.990000	-0.171133
3866_Position 104_00010.hld	3386.124105	1049662.546578	6779.568100	279148634.195515	3520.984726	3502.244616	359.516728	3.760228	0.061304	3076.301737	2.751083	-133.124000	-60.940000	-0.155064
3866_Position 104_00011.hld	3386.781095	989759.179336	6537.692573	279257119.111963	3521.267747	3500.325649	346.622856	3.544258	0.051286	3079.929181	2.776860	-133.074000	-60.940000	-0.153926
3866_Position 104_00012.hld	3393.634880	1000337.695174	6998.736067	280390104.105943	3521.248275	3500.833274	370.316534	3.567664	0.023953	3084.930157	2.909814	-133.024000	-60.940000	-0.133896
3866_Position 104_00013.hld	3390.501991	980770.286828	6646.323734	279871927.389528	3521.995244	3501.176364	351.995126	3.504354	0.050575	3089.810067	2.787680	-132.974000	-60.940000	-0.132717
3866_Position 104_00014.hld	3385.540061	1033030.546251	6661.049222	279052212.089914	3521.229002	3501.854005	353.292759	3.701926	0.082691	3082.239250	2.705704	-132.924000	-60.940000	-0.126573
3866_Position 104_00015.hld	3386.689995	1046175.330896	6764.908240	279242074.894615	3522.500735	3502.675529	358.679297	3.746482	0.043500	3069.717468	2.799647	-133.124000	-60.890000	-0.096016
3866_Position 104_00016.hld	3383.064559	998109.898569	6344.464156	278643707.522734	3521.321503	3501.054417	336.748102	3.582029	0.159957	3091.785005	2.601512	-133.074000	-60.890000	-0.101603
3866_Position 104_00017.hld	3381.676183	1061152.312400	6589.349584	278414730.553740	3521.409846	3502.456576	349.889792	3.811409	0.098482	3072.419740	2.670364	-133.024000	-60.890000	-0.104044
3866_Position 104_00018.hld	3379.417887	1107069.976875	6709.822832	278042484.028089	3521.352774	3503.162209	356.525257	3.981658	0.110548	3065.785161	2.650892	-132.974000	-60.890000	-0.070655
3866_Position 104_00019.hld	3380.348520	1079310.265138	6619.201754	278195854.826344	3521.601984	3502.641619	351.613159	3.879678	0.143119	3076.220329	2.615160	-132.924000	-60.890000	-0.049217
3866_Position 104_00020.hld	3391.784661	1058328.882517	7156.363566	280084021.637982	3521.311308	3502.699465	378.863753	3.778612	0.063452	3093.743058	2.765341	-133.124000	-60.840000	-0.091638
3866_Position 104_00021.hld	3387.219223	1076269.189755	6981.965134	279329476.348324	3520.105516	3502.831644	370.129858	3.853046	0.033443	3064.723590	2.842091	-133.074000	-60.840000	-0.085067
3866_Position 104_00022.hld	3389.343258	1038153.758606	6937.404846	279680395.866044	3520.899936	3501.577636	367.536821	3.711929	0.029130	3072.319893	2.868491	-133.024000	-60.840000	-0.099243
3866_Position 104_00023.hld	3392.709212	1016325.848506	6965.946800	280236949.538851	3521.145546	3502.133588	368.682296	3.626666	0.018907	3073.610376	2.937119	-132.974000	-60.840000	-0.064027
3866_Position 104_00024.hld	3390.246892	1019611.444471	6874.070979	279829755.527140	3522.149144	3501.492264	364.084252	3.643685	0.076406	3096.210469	2.732350	-132.924000	-60.840000	-0.045842