Thu Jun 16 11:35:07 2022

Number of Points = 9928

Depth (nm)	Load (N)	Time (s)
1.297884	109.408118	0.000000
1.106092	103.536236	0.005005
1.049896	106.095977	0.010010
1.118298	97.623205	0.015014
0.714894	90.437900	0.020019
0.305075	81.145531	0.025024
0.311415	76.870969	0.030029
-0.062687	56.302637	0.035034
-0.518645	50.103199	0.040038
-1.283500	51.889499	0.045043
-1.157699	28.379617	0.050048
-1.518750	35.357499	0.055053
-1.511239	33.463949	0.060058
-1.766513	24.676238	0.065062
-2.123039	23.201948	0.070067
-2.484420	3.828247	0.075072
-2.348642	16.031550	0.080077
-2.836328	2.607483	0.085082
-2.902506	-7.839432	0.090086
-3.377951	4.309888	0.095091
-4.244434	-9.657298	0.100096
-4.501380	-5.355138	0.105101
-4.854385	-3.206285	0.110106
-4.744597	-13.326435	0.115110
-4.695383	-4.237719	0.120115
-5.001525	-2.761433	0.125120
-4.999817	-4.173776	0.130125
-5.615265	-3.989831	0.135130
-5.706374	-1.917702	0.140134
-6.371240	-1.022194	0.145139
-6.563301	-7.750790	0.150144
-6.342761	-5.058140	0.155149
-7.054096	-3.441495	0.160154
-7.576162	-0.876996	0.165158
-8.088989	1.436483	0.170163
-8.230047	0.869414	0.175168
-8.417076	-7.086961	0.180173
-8.357058	-2.861056	0.185178
-8.206789	-7.826472	0.190182
-8.357495	-6.243086	0.195187
-8.376883	-14.693495	0.200192
-9.129778	-3.481307	0.205197
-9.454972	-5.093362	0.210202
-9.788603	-10.863921	0.215206
-10.057586	-3.335793	0.220211
-10.001144	-21.184967	0.225216
-10.060119	-4.819689	0.230221
-11.086249	-0.300046	0.235226
-11.046230	-11.168788	0.240230
-11.777247	-7.513778	0.245235
-11.414211	-14.222529	0.250240
-11.759137	-13.422612	0.255245
-11.617046	-4.083080	0.260250
-11.613885	-11.534408	0.265254
-12.456114	-6.881395	0.270259
-13.056863	-11.986296	0.275264
-13.021456	-12.670426	0.280269
-13.452216	-7.125717	0.285274
-13.209666	-9.343605	0.290278
-13.455792	-4.472625	0.295283
-14.406809	4.548672	0.300288
-14.483588	-8.689455	0.305293
-14.998979	-9.810749	0.310298
-14.897658	-17.981494	0.315302
-14.915454	-3.269537	0.320307
-15.236023	-14.109070	0.325312
-14.881830	-12.863848	0.330317
-15.654357	-9.264721	0.335322
-15.974797	-3.676090	0.340326
-16.223804	-15.211805	0.345331
-16.251274	-9.177539	0.350336
-16.598778	-1.579709	0.355341
-16.975117	-9.428636	0.360346
-17.316910	-10.162302	0.365350
-17.592737	-8.230317	0.370355
-17.953839	-13.909125	0.375360
-18.213260	-11.900831	0.380365
-18.373491	-0.345607	0.385370
-18.098838	-8.699887	0.390374
-18.500795	-1.704016	0.395379
-18.772587	-12.275974	0.400384
-19.347050	-13.699839	0.405389
-19.941379	-9.315091	0.410394
-19.513394	-8.968953	0.415398
-19.879605	2.688482	0.420403
-19.611246	-6.680885	0.425408
-20.376632	1.154506	0.430413
-20.942726	1.444142	0.435418
-21.004729	-4.767893	0.440422
-21.308719	-3.309720	0.445427
-21.061216	-1.540775	0.450432
-21.998754	-8.084019	0.455437
-22.899016	0.825303	0.460442
-22.462280	-1.230826	0.465446
-23.003267	-3.809531	0.470451
-23.036949	-3.385124	0.475456
-22.617530	-6.695130	0.480461
-22.931400	-1.130867	0.485466
-22.723573	-5.739102	0.490470
-23.073276	1.054677	0.495475
-24.069631	-5.216824	0.500480
-24.291208	4.676570	0.505485
-24.166741	-2.131071	0.510490
-24.810673	-9.829919	0.515494
-25.629086	-9.837852	0.520499
-25.943513	-12.372017	0.525504
-25.435399	-9.431330	0.530509
-26.210876	-4.167143	0.535514
-26.181710	-8.505334	0.540518
-25.858736	-6.982670	0.545523
-25.951664	-6.932331	0.550528
-26.230863	-10.737937	0.555533
-27.117298	-0.369851	0.560538
-27.014306	-7.566580	0.565542
-27.412599	-1.295328	0.570547
-27.578391	-5.596072	0.575552
-28.329154	-11.231201	0.580557
-28.866346	-4.189206	0.585562
-28.998959	-17.205400	0.590566
-29.036806	3.275545	0.595571
-29.418898	-1.888183	0.600576
-28.973055	-11.056129	0.605581
-29.238373	6.627227	0.610586
-29.134819	3.052151	0.615590
-29.390333	-1.791945	0.620595
-30.109045	4.115454	0.625600
-30.467956	-8.038511	0.630605
-30.682496	-4.959751	0.635610
-30.706675	-18.932054	0.640614
-31.645066	-3.323820	0.645619
-31.733543	-10.012312	0.650624
-31.994638	-5.434324	0.655629
-32.402602	-5.908843	0.660634
-32.322090	-18.044857	0.665638
-32.490445	-2.473713	0.670643
-32.458071	-3.043695	0.675648
-32.526098	0.198294	0.680653
-33.369073	-5.369113	0.685658
-33.571757	-16.093265	0.690662
-33.810035	-3.571864	0.695667
-33.554187	-8.401124	0.700672
-34.469718	1.681436	0.705677
-35.060316	-1.104725	0.710682
-35.254572	-10.851538	0.715686
-35.360640	0.486477	0.720691
-35.423666	-5.445805	0.725696
-35.315892	-9.347524	0.730701
-35.863458	-3.494950	0.735706
-35.511497	-6.285350	0.740710
-35.649338	1.413085	0.745715
-36.239416	-8.547600	0.750720
-36.675647	-0.377322	0.755725
-36.892324	-4.276920	0.760730
-36.806645	-3.788581	0.765734
-37.958738	2.609617	0.770739
-38.490893	4.623427	0.775744
-38.558150	-2.887986	0.780749
-38.727207	-2.864231	0.785754
-38.515899	1.928490	0.790758
-38.764380	-10.353622	0.795763
-38.775088	-3.181697	0.800768
-38.820698	-3.857963	0.805773
-39.258545	-4.417022	0.810778
-39.875101	-9.398556	0.815782
-40.230837	8.187772	0.820787
-40.401708	4.890081	0.825792
-40.470798	-8.471643	0.830797
-40.365020	-2.641609	0.835802
-40.895290	-4.752298	0.840806
-41.647248	-9.446276	0.845811
-41.898209	-4.217965	0.850816
-41.834171	-7.061803	0.855821
-41.940762	0.600391	0.860826
-41.811880	-0.131053	0.865830
-42.583897	-6.388523	0.870835
-43.091588	-6.581874	0.875840
-43.150055	-1.199217	0.880845
-43.418712	-7.829913	0.885850
-43.506475	1.988584	0.890854
-43.669771	-10.224835	0.895859
-43.639933	-14.307625	0.900864
-44.059162	-6.300865	0.905869
-44.947175	-9.382170	0.910874
-44.741977	-8.448041	0.915878
-45.105505	-4.609891	0.920883
-45.289883	-7.891239	0.925888
-45.207576	-12.528153	0.930893
-45.785186	0.542003	0.935898
-46.221905	-6.812852	0.940902
-46.574520	0.311402	0.945907
-46.639675	-1.430638	0.950912
-46.651348	-5.261713	0.955917
-46.847802	3.046614	0.960922
-46.956655	-2.800554	0.965926
-47.634319	-0.166240	0.970931
-47.887864	-2.836348	0.975936
-47.992506	-0.039843	0.980941
-48.174682	-3.137075	0.985946
-48.168118	-15.741998	0.990950
-49.306841	0.238811	0.995955
-49.310158	-9.860967	1.000960
-49.209341	-5.791761	1.005965
-49.966540	7.100515	1.010970
-49.685118	-13.823073	1.015974
-49.779706	-4.205986	1.020979
-50.012053	-3.512670	1.025984
-50.685420	-19.836309	1.030989
-51.303926	-7.737150	1.035994
-51.336933	-14.079261	1.040998
-51.309369	-12.161407	1.046003
-51.242914	-10.042711	1.051008
-51.476652	-16.187982	1.056013
-52.355724	-2.395194	1.061018
-52.603034	-9.387034	1.066022
-52.925849	-8.084679	1.071027
-52.810776	-7.080904	1.076032
-52.781537	-4.825539	1.081037
-52.844510	-5.713111	1.086042
-53.041326	-7.714354	1.091046
-54.079794	-5.519102	1.096051
-54.563565	-5.469082	1.101056
-54.473964	-4.224823	1.106061
-54.545419	-5.685548	1.111066
-54.349824	-5.240730	1.116070
-54.850006	2.417652	1.121075
-55.483672	-12.666369	1.126080
-56.002297	-5.502449	1.131085
-56.182243	-2.696459	1.136090
-56.308867	-4.298808	1.141094
-56.056009	-6.565557	1.146099
-56.351326	-3.772266	1.151104
-56.344511	-17.397794	1.156109
-57.309518	-5.671790	1.161114
-57.586457	-7.390469	1.166118
-57.778017	-9.036739	1.171123
-57.965152	-7.798340	1.176128
-58.017817	-11.200108	1.181133
-58.343388	-9.860599	1.186138
-58.065726	-10.085286	1.191142
-59.042517	1.931329	1.196147
-59.215185	-2.448483	1.201152
-59.517998	-7.143980	1.206157
-59.904282	0.220829	1.211162
-59.373549	-17.523626	1.216166
-59.346467	-13.279064	1.221171
-60.285260	-1.617963	1.226176
-60.828101	-2.164008	1.231181
-61.390650	1.907696	1.236186
-60.968909	-9.856463	1.241190
-61.120654	-2.792341	1.246195
-61.317215	-9.638175	1.251200
-62.268307	-8.407983	1.256205
-62.563581	-4.065552	1.261210
-62.717246	-15.181661	1.266214
-62.718183	-7.473401	1.271219
-63.130057	-10.220728	1.276224
-62.654176	-19.333356	1.281229
-63.214163	-4.753474	1.286234
-62.868137	-14.936731	1.291238
-63.801111	-6.949540	1.296243
-64.605863	-6.917304	1.301248
-64.549137	-8.281323	1.306253
-64.792122	-9.655098	1.311258
-64.546790	-1.497823	1.316262
-64.586793	-8.101788	1.321267
-65.502088	-0.681909	1.326272
-65.702566	-8.935367	1.331277
-66.285700	-2.730740	1.336282
-66.195416	-5.726993	1.341286
-66.672173	-3.789323	1.346291
-66.311769	-10.840360	1.351296
-66.242261	-12.716723	1.356301
-67.245929	-7.841692	1.361306
-67.594240	-4.936156	1.366310
-67.902760	-6.393808	1.371315
-67.940046	-4.331265	1.376320
-67.974414	-9.244460	1.381325
-68.024059	-3.475557	1.386330
-68.454221	-14.604371	1.391334
-69.289608	-15.098515	1.396339
-69.730172	-15.575239	1.401344
-69.598311	-7.430389	1.406349
-69.516106	-1.384753	1.411354
-69.559795	-17.100674	1.416358
-70.069799	-6.955805	1.421363
-70.265722	4.101495	1.426368
-70.411062	-4.597912	1.431373
-70.952154	-1.673241	1.436378
-71.114757	-9.461298	1.441382
-71.237555	-3.101311	1.446387
-71.623630	-10.074851	1.451392
-71.415314	-8.161912	1.456397
-72.269332	11.925539	1.461402
-72.116808	-0.374607	1.466406
-72.531569	4.801855	1.471411
-72.712633	-7.607411	1.476416
-72.779015	-1.084203	1.481421
-73.416124	8.326001	1.486426
-73.927026	-4.437967	1.491430
-74.275191	-0.135233	1.496435
-74.498396	-0.141890	1.501440
-74.279345	-3.954370	1.506445
-74.680898	-3.122795	1.511450
-74.527957	2.475896	1.516454
-75.095112	-8.775004	1.521459
-75.536767	-14.924878	1.526464
-75.889137	-6.483357	1.531469
-76.115550	4.126264	1.536474
-75.866193	-11.735859	1.541478
-76.129567	-8.076546	1.546483
-76.564345	-2.273785	1.551488
-77.292801	-2.710525	1.556493
-77.782385	-2.699498	1.561498
-77.642876	-6.153152	1.566502
-77.745501	-19.806263	1.571507
-77.984003	-6.533689	1.576512
-77.655643	-13.960130	1.581517
-77.961135	-4.959891	1.586522
-78.118075	-3.423519	1.591526
-78.859936	-6.547322	1.596531
-79.136279	-12.629614	1.601536
-79.071092	-9.884461	1.606541
-79.505805	-11.519548	1.611546
-80.153640	-7.869500	1.616550
-80.645976	-8.469468	1.621555
-80.980821	-15.700175	1.626560
-81.177813	-14.826445	1.631565
-81.144559	1.790145	1.636570
-80.832113	-12.850129	1.641574
-80.971988	-8.726545	1.646579
-81.447741	-6.647177	1.651584
-81.408086	-18.582974	1.656589
-82.252717	-3.695507	1.661594
-82.170666	-11.166182	1.666598
-82.629939	-10.406159	1.671603
-82.775906	-6.955269	1.676608
-82.876508	-11.527324	1.681613
-83.748024	-2.227450	1.686618
-84.012534	-14.722655	1.691622
-84.121350	-7.805718	1.696627
-84.403401	-2.670429	1.701632
-84.418303	-9.591270	1.706637
-84.672561	-1.192302	1.711642
-84.285925	-10.659048	1.716646
-84.901613	-4.244237	1.721651
-85.526679	-5.344537	1.726656
-85.634273	-9.543515	1.731661
-85.796207	-3.944581	1.736666
-85.895495	-8.906434	1.741670
-86.294749	-8.959661	1.746675
-87.007154	-17.037350	1.751680
-87.137219	-12.751822	1.756685
-87.820997	-8.598918	1.761690
-87.806039	-11.554703	1.766694
-87.939900	-9.824544	1.771699
-87.993161	-11.668581	1.776704
-88.042836	-19.904435	1.781709
-88.390322	-6.042650	1.786714
-88.136465	-5.742221	1.791718
-88.422726	-11.152428	1.796723
-89.185761	-7.050352	1.801728
-89.181627	-5.428038	1.806733
-89.561767	-6.631363	1.811738
-89.786294	-7.160760	1.816742
-90.266932	-2.755730	1.821747
-90.801186	-7.219317	1.826752
-90.491568	-8.333612	1.831757
-91.115447	-9.922636	1.836762
-91.140151	-11.897866	1.841766
-90.864817	-8.996453	1.846771
-91.688581	-15.749079	1.851776
-92.057471	-14.499286	1.856781
-92.430662	-3.854660	1.861786
-92.474582	-11.222436	1.866790
-92.651837	-9.878729	1.871795
-92.603023	-4.062667	1.876800
-93.102657	-13.678991	1.881805
-93.860385	-7.360569	1.886810
-93.653141	-8.659493	1.891814
-94.256503	-15.755651	1.896819
-94.642191	-4.382185	1.901824
-94.168896	-13.861673	1.906829
-94.415488	-9.067370	1.911834
-94.463079	-11.830802	1.916838
-95.091176	-14.036004	1.921843
-95.752538	-13.125184	1.926848
-95.867222	-14.561301	1.931853
-95.825843	-10.261293	1.936858
-95.602684	-9.795678	1.941862
-96.373213	-8.666352	1.946867
-97.234206	-12.331107	1.951872
-97.250756	-20.268188	1.956877
-97.383753	-8.333523	1.961882
-97.617858	3.429337	1.966886
-97.718472	-12.292665	1.971891
-97.185640	-20.292725	1.976896
-97.941129	-21.172287	1.981901
-98.388387	-5.961707	1.986906
-98.649952	-12.658382	1.991910
-98.718378	-5.578438	1.996915
-99.000336	-5.464516	2.006912
-99.007963	-8.513292	2.016909
-98.857202	-8.726316	2.026906
-97.853076	-10.711174	2.036902
-97.767304	-14.828766	2.046899
-96.748181	-18.413015	2.056896
-96.251018	-8.877730	2.066893
-96.163038	-4.823488	2.076890
-95.285019	-9.588882	2.086886
-95.031529	-10.281517	2.096883
-94.436022	-8.657656	2.106880
-93.537528	-5.081369	2.116877
-93.302363	-11.276977	2.126874
-93.263058	-10.252743	2.136870
-92.351209	-10.585628	2.146867
-92.234760	-10.630094	2.156864
-91.248168	-14.143229	2.166861
-90.582407	-6.327745	2.176858
-90.410304	-9.110876	2.186854
-90.144930	-6.681582	2.196851
-89.239763	-16.701772	2.206848
-88.686308	-8.599295	2.216845
-88.530908	-20.625344	2.226842
-87.619878	-6.881370	2.236838
-86.895041	-14.005876	2.246835
-87.131056	-13.673181	2.256832
-86.687967	-5.671293	2.266829
-85.701366	-10.109448	2.276826
-85.438621	-10.724885	2.286822
-85.114179	-11.716544	2.296819
-84.163937	-6.483145	2.306816
-84.008490	-1.937710	2.316813
-83.385248	-3.243679	2.326810
-82.705118	-6.272278	2.336806
-82.483011	-6.099753	2.346803
-81.910157	-7.199787	2.356800
-80.893280	-8.195995	2.366797
-81.095460	-2.510118	2.376794
-80.692902	-6.341898	2.386790
-79.531605	-10.813666	2.396787
-79.073309	-9.824255	2.406784
-79.176950	-3.382310	2.416781
-78.432243	-10.481357	2.426778
-77.808001	-2.393685	2.436774
-77.208557	-10.160920	2.446771
-76.349524	-2.970641	2.456768
-76.720685	-6.508895	2.466765
-76.296200	-1.954139	2.476762
-74.908164	-4.682588	2.486758
-74.458173	-3.568132	2.496755
-74.436075	-9.742208	2.506752
-74.204656	-9.264365	2.516749
-73.473319	-7.911430	2.526746
-73.142521	-12.738649	2.536742
-71.974744	-3.593142	2.546739
-71.952426	-16.820236	2.556736
-71.362725	-10.435887	2.566733
-70.300061	-9.036510	2.576730
-70.126376	-9.386427	2.586726
-70.041801	-12.949030	2.596723
-69.732127	-15.518369	2.606720
-68.871922	-12.605376	2.616717
-68.311226	-16.973779	2.626714
-67.444095	-4.386210	2.636710
-67.109630	-11.552289	2.646707
-66.939172	-12.446835	2.656704
-66.642494	-11.315882	2.666701
-65.682845	-6.099788	2.676698
-65.220870	-8.707190	2.686694
-64.895315	-12.606203	2.696691
-63.822959	-9.191010	2.706688
-63.762080	-7.565467	2.716685
-63.744055	-17.167100	2.726682
-63.059036	-9.885634	2.736678
-62.084659	-12.555247	2.746675
-61.833376	-10.148219	2.756672
-61.181457	-3.581479	2.766669
-60.747790	-5.839809	2.776666
-60.615847	-8.207653	2.786662
-59.468826	-14.841754	2.796659
-58.860927	-9.083558	2.806656
-58.846403	-2.500723	2.816653
-58.736651	-9.962206	2.826650
-57.531980	-12.406681	2.836646
-57.226186	-8.422613	2.846643
-57.110743	-11.705883	2.856640
-55.989799	0.085765	2.866637
-55.559518	-5.021146	2.876634
-55.480167	-2.579528	2.886630
-54.910911	-10.569607	2.896627
-54.322807	-13.515329	2.906624
-54.095631	-11.046877	2.916621
-52.923215	-7.290785	2.926618
-52.458577	-12.601176	2.936614
-52.189536	-13.397233	2.946611
-52.088878	-9.635496	2.956608
-51.573678	-12.508519	2.966605
-50.782447	-5.434159	2.976602
-49.864663	-9.293450	2.986598
-49.405137	-9.406122	2.996595
-49.085509	-2.038926	3.006592
-49.024757	-2.133504	3.016589
-48.738744	-5.916438	3.026586
-48.104400	-11.365608	3.036582
-47.020559	-13.991128	3.046579
-46.381911	-3.230841	3.056576
-46.205518	-13.728105	3.066573
-45.952386	-13.766711	3.076570
-45.709273	-13.345770	3.086566
-44.672782	-10.449855	3.096563
-44.265173	-8.044855	3.106560
-43.174458	-13.047300	3.116557
-42.879028	-11.241823	3.126554
-42.897451	2.060783	3.136550
-42.842571	-4.494472	3.146547
-41.990705	-6.021555	3.156544
-41.199012	-11.099637	3.166541
-40.368200	-1.196850	3.176538
-39.972417	-3.898512	3.186534
-40.154155	-9.095908	3.196531
-39.505621	-9.435102	3.206528
-38.720727	-12.835923	3.216525
-38.508512	-15.190116	3.226522
-36.997151	-2.363574	3.236518
-37.307387	-6.813459	3.246515
-36.728828	-6.085533	3.256512
-36.475771	-10.790409	3.266509
-35.390476	-7.504378	3.276506
-34.935305	-15.680666	3.286502
-34.651118	-8.021649	3.296499
-34.384152	-11.392833	3.306496
-33.706020	-5.657500	3.316493
-33.191886	-4.270688	3.326490
-33.053745	-6.717049	3.336486
-31.910222	-7.769543	3.346483
-31.646419	-3.782186	3.356480
-31.613211	-11.101027	3.366477
-30.602918	-10.626106	3.376474
-30.033449	-10.813892	3.386470
-29.754264	-11.245401	3.396467
-29.173147	-9.553911	3.406464
-28.618439	-14.254210	3.416461
-28.346998	-8.388793	3.426458
-27.909388	-16.493774	3.436454
-26.737047	-9.309581	3.446451
-26.768716	-2.822482	3.456448
-26.497073	-7.820495	3.466445
-25.645210	-9.219410	3.476442
-25.163776	-10.101438	3.486438
-24.847244	-13.015218	3.496435
-23.834191	-4.500959	3.506432
-23.341475	-7.424496	3.516429
-23.364120	-2.130413	3.526426
-23.074712	-8.111846	3.536422
-22.571578	-10.814603	3.546419
-21.843042	-18.003429	3.556416
-20.916193	-3.674458	3.566413
-20.970982	-6.648915	3.576410
-20.043977	-4.393017	3.586406
-19.243868	-11.825312	3.596403
-19.114467	-8.693546	3.606400
-18.949029	-6.071361	3.616397
-18.208400	-3.713887	3.626394
-17.579835	-8.878753	3.636390
-17.538359	-5.996097	3.646387
-16.556687	-7.800468	3.656384
-16.008063	-9.301487	3.666381
-16.070171	-2.789750	3.676378
-15.230457	-4.266223	3.686374
-14.435148	-2.632699	3.696371
-14.163129	-9.612337	3.706368
-13.688891	-7.543132	3.716365
-12.934792	-2.673455	3.726362
-12.630645	-2.313124	3.736358
-12.589734	-1.933196	3.746355
-11.394292	-1.102247	3.756352
-10.678317	-4.871830	3.766349
-10.693734	0.672058	3.776346
-10.771956	2.627845	3.786342
-10.010640	-5.817839	3.796339
-8.820451	0.918463	3.806336
-7.979134	-10.773832	3.816333
-8.544720	-3.398978	3.826330
-8.109264	-7.203300	3.836326
-6.912025	-2.164797	3.846323
-6.405199	-2.707416	3.856320
-6.143442	-6.121994	3.866317
-5.880196	1.491498	3.876314
-5.115501	9.244527	3.886310
-4.799604	5.746569	3.896307
-4.331263	8.628571	3.906304
-3.781246	11.318729	3.916301
-3.341040	13.299079	3.926298
-2.935929	29.402400	3.936294
-2.501058	32.107145	3.946291
-1.773487	38.832597	3.956288
-1.690714	51.493895	3.966285
-1.175583	70.243362	3.976282
-0.797984	87.386256	3.986278
0.087869	105.586332	3.996275
0.000000	112.582077	4.001280
0.396129	119.070538	4.006285
0.754052	138.688551	4.011290
1.166175	126.380614	4.016294
0.884158	145.959173	4.021299
1.253237	148.356597	4.026304
1.260915	138.219482	4.031309
0.852204	144.829911	4.036314
0.856884	133.158733	4.041318
0.927692	142.780941	4.046323
1.201885	145.401119	4.051328
1.161747	138.016164	4.056333
0.842057	147.537564	4.061338
1.195842	149.449770	4.066342
1.272833	143.309707	4.071347
0.984415	139.017642	4.076352
1.224032	132.642449	4.081357
1.035745	150.234321	4.086362
0.899977	138.763038	4.091366
0.958466	153.302326	4.096371
0.968107	166.085963	4.101376
1.233199	163.952818	4.106381
1.591425	173.844522	4.111386
1.813342	165.195994	4.116390
1.163781	158.843431	4.121395
1.130680	158.380451	4.126400
1.589667	157.230710	4.131405
1.506507	164.517487	4.136410
1.563320	138.438441	4.141414
1.444979	146.918717	4.146419
1.092784	150.701463	4.151424
1.174510	147.935964	4.156429
1.190642	162.393077	4.161434
1.442806	177.930134	4.166438
1.359233	178.170908	4.171443
1.417206	168.236976	4.176448
1.813560	175.666486	4.181453
1.527707	182.831979	4.186458
1.613527	170.668890	4.191462
1.641658	175.256847	4.196467
1.633082	171.843706	4.201472
1.325938	150.845493	4.206477
1.187368	167.596726	4.211482
1.754331	165.575289	4.216486
1.413086	175.144663	4.221491
1.385788	172.922904	4.226496
1.423846	174.619148	4.231501
1.372984	175.810969	4.236506
1.507755	167.804972	4.241510
1.699752	171.560041	4.246515
1.706487	174.039743	4.251520
1.539106	175.619589	4.256525
1.333235	180.209716	4.261530
1.696411	169.813267	4.266534
1.851345	182.409831	4.271539
1.805639	179.945564	4.276544
1.972352	171.817775	4.281549
1.761653	186.279940	4.286554
1.560683	183.444247	4.291558
1.864208	177.748758	4.296563
1.717079	178.695153	4.301568
1.919553	180.005223	4.306573
1.400376	172.395562	4.311578
1.631874	177.364950	4.316582
1.583844	180.977966	4.321587
1.529637	176.687733	4.326592
1.942710	171.894191	4.331597
1.344537	186.147807	4.336602
2.013318	180.757173	4.341606
1.729947	182.562473	4.346611
1.904558	202.431255	4.351616
2.059427	197.862492	4.356621
2.115585	197.391962	4.361626
2.052287	186.094137	4.366630
1.561170	188.400602	4.371635
1.763457	197.986417	4.376640
1.928161	198.656841	4.381645
2.071826	207.547959	4.386650
2.389337	205.279670	4.391654
1.979902	205.950465	4.396659
2.066716	195.157206	4.401664
1.913645	188.482456	4.406669
1.669088	197.657131	4.411674
2.096417	193.004078	4.416678
2.246174	204.813170	4.421683
2.363882	205.716885	4.426688
2.477152	195.762452	4.431693
2.465648	186.553063	4.436698
2.161214	188.301962	4.441702
2.273666	180.544901	4.446707
1.645358	176.196135	4.451712
1.742252	181.141006	4.456717
1.930732	202.375140	4.461722
2.057579	200.620386	4.466726
2.128153	206.121388	4.471731
2.352758	203.952507	4.476736
2.523260	202.872635	4.481741
2.291457	213.822470	4.486746
2.471813	201.649061	4.491750
2.123587	189.184281	4.496755
2.020605	197.730513	4.501760
2.288176	197.917796	4.506765
2.281976	211.684416	4.511770
2.537418	197.960481	4.516774
2.547036	196.391629	4.521779
2.081474	191.307231	4.526784
2.574448	189.498188	4.531789
2.321372	201.987676	4.536794
2.387670	197.664302	4.541798
2.125231	197.485759	4.546803
2.506568	205.292848	4.551808
2.565623	200.432905	4.556813
2.206943	213.079056	4.561818
2.718041	210.345780	4.566822
2.691698	214.668492	4.571827
2.374737	192.875506	4.576832
2.350063	181.881273	4.581837
2.369999	198.249414	4.586842
2.587753	204.541175	4.591846
2.415841	205.632743	4.596851
2.190139	207.978119	4.601856
2.731060	208.973096	4.606861
2.380319	209.908846	4.611866
2.619147	207.608968	4.616870
2.470173	206.874599	4.621875
2.626822	197.051408	4.626880
2.674102	210.033174	4.631885
2.643037	213.837745	4.636890
2.767762	203.470715	4.641894
2.789554	210.631058	4.646899
2.438314	208.167852	4.651904
3.090500	198.513548	4.656909
2.324939	208.060131	4.661914
2.642123	199.574996	4.666918
2.302487	195.833583	4.671923
2.428532	215.117397	4.676928
2.476620	197.461921	4.681933
2.319863	205.322913	4.686938
3.021171	201.166883	4.691942
2.303647	207.305999	4.696947
2.528389	204.289555	4.701952
2.395021	212.838844	4.706957
2.269053	218.488053	4.711962
2.713088	217.937540	4.716966
2.766437	238.988459	4.721971
2.988212	233.754549	4.726976
2.983735	230.202797	4.731981
2.945968	243.842466	4.736986
3.164800	227.083725	4.741990
2.923989	241.769240	4.746995
2.905262	237.111064	4.752000
3.073257	240.789812	4.757005
2.615040	231.926900	4.762010
3.170076	232.958613	4.767014
3.160687	235.570326	4.772019
3.103405	230.502990	4.777024
3.006286	215.459691	4.782029
2.548219	211.806313	4.787034
2.955122	218.602613	4.792038
2.885374	222.192494	4.797043
2.811801	245.645029	4.802048
2.997692	239.472823	4.807053
3.137200	237.718537	4.812058
3.127721	236.631016	4.817062
3.123846	231.528611	4.822067
3.140817	228.410849	4.827072
3.343186	251.621864	4.832077
3.060136	244.306005	4.837082
3.230151	236.931358	4.842086
3.413582	238.643046	4.847091
3.374058	238.958721	4.852096
3.342041	221.826795	4.857101
2.984537	224.375677	4.862106
3.185551	212.874332	4.867110
2.906181	215.327726	4.872115
2.908926	230.248128	4.877120
3.069444	238.540901	4.882125
3.348453	249.535386	4.887130
3.020212	241.954612	4.892134
2.749227	247.689554	4.897139
3.112197	237.929712	4.902144
3.369566	233.435550	4.907149
3.249137	247.955465	4.912154
3.151433	235.397945	4.917158
3.142926	239.550991	4.922163
2.808947	245.780540	4.927168
3.426545	235.783382	4.932173
3.398523	244.568822	4.937178
3.424111	236.387174	4.942182
3.192572	251.091488	4.947187
3.171169	244.412713	4.952192
3.557268	261.951719	4.957197
3.522898	267.886705	4.962202
3.188533	256.477158	4.967206
3.380151	270.081015	4.972211
3.320351	270.426678	4.977216
3.808854	272.201013	4.982221
3.313087	273.873119	4.987226
3.870073	262.361448	4.992230
3.651102	263.777379	4.997235
3.216236	254.699277	5.002240
3.585891	253.993637	5.007245
3.532708	274.046067	5.012250
3.872281	270.326957	5.017254
3.604353	261.837558	5.022259
3.141250	249.505955	5.027264
3.551559	265.850697	5.032269
3.413118	276.650879	5.037274
3.639618	275.448294	5.042278
3.760376	271.093604	5.047283
3.411486	268.261523	5.052288
3.795130	270.020730	5.057293
3.660211	272.926271	5.062298
3.422893	268.571563	5.067302
3.469173	275.074794	5.072307
3.501196	277.924532	5.077312
3.469875	272.525160	5.082317
3.605576	261.513937	5.087322
3.714361	261.232905	5.092326
3.680794	272.663915	5.097331
3.520714	272.450400	5.102336
3.843634	264.869538	5.107341
3.511410	274.512066	5.112346
3.851568	262.871671	5.117350
3.763304	276.292512	5.122355
3.739380	277.909333	5.127360
3.889380	275.603999	5.132365
3.687895	287.292240	5.137370
4.071857	294.964772	5.142374
3.898265	281.333466	5.147379
3.789053	277.259765	5.152384
4.184903	286.421495	5.157389
3.646659	300.657322	5.162394
4.215631	290.489797	5.167398
4.047723	287.748854	5.172403
3.804162	292.213835	5.177408
4.152807	275.068269	5.182413
3.596591	275.613763	5.187418
4.332279	288.431517	5.192422
3.964471	288.364896	5.197427
3.724402	282.743516	5.202432
4.252944	297.066157	5.207437
4.330666	298.133841	5.212442
3.992694	284.832765	5.217446
4.157401	271.433930	5.222451
4.029407	280.152154	5.227456
3.800987	280.218767	5.232461
4.125866	293.328065	5.237466
4.168774	298.867315	5.242470
3.965838	305.718856	5.247475
4.463791	305.645700	5.252480
4.330616	313.581281	5.257485
4.284338	297.594941	5.262490
4.399299	275.168322	5.267494
4.120238	273.634442	5.272499
3.803317	283.427756	5.277504
4.279795	285.840700	5.282509
4.410519	307.947557	5.287514
4.485411	304.350609	5.292518
4.328949	283.946372	5.297523
3.863615	276.910120	5.302528
4.118670	281.678832	5.307533
4.438681	314.954016	5.312538
4.561882	298.266051	5.317542
4.345900	288.117852	5.322547
4.208165	287.616124	5.327552
4.641994	296.781943	5.332557
4.307103	294.157482	5.337562
4.293230	285.022516	5.342566
4.249616	286.738780	5.347571
4.400630	303.680952	5.352576
4.473977	302.742913	5.357581
4.579281	317.008942	5.362586
4.494937	304.347346	5.367590
4.419536	298.598317	5.372595
4.386810	290.852268	5.377600
4.495721	304.128280	5.382605
4.473931	307.626891	5.387610
4.361659	320.017340	5.392614
4.719081	312.913373	5.397619
4.351688	310.619744	5.402624
4.493588	312.276052	5.407629
4.565125	315.681207	5.412634
4.510122	315.791575	5.417638
4.597757	312.069004	5.422643
4.300623	323.531473	5.427648
4.559375	303.516944	5.432653
4.274945	313.954353	5.437658
4.599068	314.463576	5.442662
4.320119	311.480135	5.447667
4.232972	324.806618	5.452672
4.302500	310.154872	5.457677
4.464760	317.729784	5.462682
4.370937	323.586320	5.467686
5.036174	327.419393	5.472691
4.755177	333.612992	5.477696
4.684863	316.320168	5.482701
4.666784	326.025153	5.487706
4.677798	319.784344	5.492710
4.595725	328.618621	5.497715
4.965412	337.141276	5.502720
4.839103	342.985530	5.507725
4.646459	345.112763	5.512730
4.732312	335.458440	5.517734
4.481353	347.613156	5.522739
4.332163	341.128202	5.527744
4.980210	342.872529	5.532749
4.508590	349.195010	5.537754
4.621854	349.160467	5.542758
4.817414	343.047295	5.547763
4.627788	350.832599	5.552768
4.786747	336.234023	5.557773
4.646072	344.982792	5.562778
4.882809	346.176326	5.567782
4.426744	356.105345	5.572787
4.683373	367.121962	5.577792
5.250132	381.413210	5.582797
5.160749	375.747754	5.587802
5.057810	375.913991	5.592806
4.895467	379.127351	5.597811
4.899974	381.786120	5.602816
5.313612	373.591571	5.607821
4.933971	371.310414	5.612826
5.355202	381.664204	5.617830
5.005430	380.803188	5.622835
5.016400	373.670420	5.627840
5.296925	370.222677	5.632845
4.870694	371.392886	5.637850
4.833426	363.815364	5.642854
5.154118	371.442354	5.647859
4.915285	362.986764	5.652864
4.789584	364.710782	5.657869
4.938157	373.522063	5.662874
5.051367	368.775450	5.667878
5.038985	371.127428	5.672883
4.524567	368.441859	5.677888
5.080766	371.237744	5.682893
5.118323	389.040290	5.687898
5.196587	397.919241	5.692902
5.271885	397.223172	5.697907
4.757320	400.514672	5.702912
5.169477	407.352710	5.707917
5.365127	401.744025	5.712922
5.665770	401.064977	5.717926
5.381958	400.012519	5.722931
5.333963	393.341822	5.727936
5.693321	392.578981	5.732941
5.483469	408.948424	5.737946
5.313274	402.317057	5.742950
5.386850	395.599730	5.747955
5.040541	401.320343	5.752960
5.553600	402.663556	5.757965
5.407378	412.461496	5.762970
5.519712	410.001361	5.767974
5.450582	399.864138	5.772979
5.233141	402.795870	5.777984
5.635998	406.781929	5.782989
5.461901	415.333524	5.787994
5.523374	400.417639	5.792998
5.483304	403.479388	5.798003
5.171545	410.881503	5.803008
5.510172	401.887104	5.808013
5.492819	412.409287	5.813018
5.350628	405.869973	5.818022
5.559468	405.213397	5.823027
5.240603	411.872823	5.828032
5.571831	395.225747	5.833037
5.214865	406.863809	5.838042
5.245843	399.467666	5.843046
5.661612	410.424769	5.848051
5.515499	433.805721	5.853056
5.933915	432.121638	5.858061
5.979707	423.700468	5.863066
5.957867	422.159877	5.868070
5.376303	411.545881	5.873075
5.394287	413.607436	5.878080
5.770499	419.919961	5.883085
5.764957	426.933386	5.888090
5.643613	435.484068	5.893094
5.890413	431.665020	5.898099
5.649668	436.653933	5.903104
6.152506	432.064197	5.908109
5.719121	445.031083	5.913114
5.956681	429.313299	5.918118
6.028369	417.464596	5.923123
5.892675	426.656242	5.928128
5.686381	409.500127	5.933133
5.834390	410.853847	5.938138
5.797373	422.397808	5.943142
5.756423	433.824435	5.948147
5.862220	434.876241	5.953152
6.093988	434.009092	5.958157
6.101152	445.111289	5.963162
5.792311	439.139346	5.968166
6.135367	440.060983	5.973171
5.965475	430.731612	5.978176
6.037197	415.633775	5.983181
5.899614	430.564440	5.988186
5.795474	425.836464	5.993190
5.718913	427.279190	5.998195
5.717698	434.451628	6.003200
6.282554	444.916588	6.008205
6.205710	441.991768	6.013210
6.089247	432.596247	6.018214
6.126457	439.416153	6.023219
5.676933	440.069510	6.028224
6.247861	441.015051	6.033229
5.889177	441.185274	6.038234
6.314302	440.208035	6.043238
6.247714	435.491313	6.048243
6.052263	447.303477	6.053248
6.365235	420.913177	6.058253
5.946997	412.527361	6.063258
5.482144	409.231696	6.068262
5.799690	419.069313	6.073267
5.635005	433.182756	6.078272
6.199159	433.521696	6.083277
6.115531	438.638154	6.088282
5.990481	440.014902	6.093286
6.437691	429.554472	6.098291
6.126219	445.151994	6.103296
6.466911	432.710790	6.108301
5.964785	430.577822	6.113306
5.700669	418.544484	6.118310
5.917035	428.226970	6.123315
6.082557	436.616693	6.128320
6.006853	436.119902	6.133325
6.169761	438.559632	6.138330
6.191778	436.427848	6.143334
6.041368	426.354058	6.148339
5.930703	427.996871	6.153344
6.159402	429.862206	6.158349
5.990115	417.377731	6.163354
5.573608	420.437664	6.168358
5.932041	431.948048	6.173363
6.207063	442.595865	6.178368
6.347296	434.633222	6.183373
6.175009	438.842590	6.188378
6.088014	425.721892	6.193382
6.030045	409.543705	6.198387
6.038502	407.496741	6.203392
6.105429	409.254635	6.208397
5.523927	411.655881	6.213402
5.899052	420.893530	6.218406
6.275558	437.632055	6.223411
5.993509	444.777507	6.228416
6.479228	433.837556	6.233421
6.194158	424.139308	6.238426
5.961079	414.315272	6.243430
5.985990	403.643577	6.248435
5.895041	412.818646	6.253440
6.157059	404.804026	6.258445
6.060243	394.732746	6.263450
5.807506	411.497982	6.268454
5.974513	398.453915	6.273459
5.447502	418.042922	6.278464
6.331924	431.873188	6.283469
6.113256	437.939819	6.288474
6.256281	421.589299	6.293478
6.477553	419.043383	6.298483
6.036131	411.575247	6.303488
6.221393	409.877902	6.308493
6.189443	409.907214	6.313498
6.095336	412.036127	6.318502
5.820568	403.355895	6.323507
5.979359	396.685356	6.328512
6.063902	398.609138	6.333517
6.178763	408.944517	6.338522
5.970765	399.485613	6.343526
6.112287	393.724574	6.348531
5.821462	404.256035	6.353536
6.252457	400.778881	6.358541
5.827176	392.514403	6.363546
5.832537	401.232854	6.368550
5.799368	397.993710	6.373555
5.633349	401.659820	6.378560
6.261974	412.376052	6.383565
6.021919	415.360752	6.388570
6.139502	406.227568	6.393574
6.244875	405.362860	6.398579
5.873824	407.966396	6.403584
6.158177	411.829779	6.408589
5.643685	405.735169	6.413594
5.793003	409.901246	6.418598
6.177983	415.078767	6.423603
5.872213	416.283431	6.428608
6.428679	411.327803	6.433613
6.021116	419.378237	6.438618
5.841962	401.382623	6.443622
6.085012	405.163349	6.448627
5.658255	411.922983	6.453632
6.236918	412.338844	6.458637
5.916332	421.605734	6.463642
5.854145	428.762693	6.468646
6.284638	441.712501	6.473651
6.162915	431.333758	6.478656
6.120537	419.669349	6.483661
5.729623	424.873283	6.488666
6.133998	415.370489	6.493670
6.110802	418.442179	6.498675
5.813220	422.267365	6.503680
6.042953	421.287493	6.508685
6.094206	432.087512	6.513690
5.990121	426.635590	6.518694
5.979948	419.886218	6.523699
6.185101	431.850987	6.528704
6.110144	410.720323	6.533709
5.835386	413.853711	6.538714
6.015524	408.090329	6.543718
6.191614	409.418789	6.548723
5.811102	417.086111	6.553728
5.945392	421.962924	6.558733
6.074123	431.746712	6.563738
5.934694	438.923839	6.568742
5.973035	439.874030	6.573747
5.699199	453.758694	6.578752
6.148724	442.986612	6.583757
6.295554	441.011979	6.588762
5.797169	444.402035	6.593766
6.249988	437.271098	6.598771
5.875312	446.965538	6.603776
6.035501	453.843658	6.608781
6.213644	449.825124	6.613786
6.153422	440.577956	6.618790
5.846976	433.855342	6.623795
6.075051	445.298390	6.628800
6.470208	438.893815	6.633805
6.175284	418.549277	6.638810
5.845133	415.772082	6.643814
5.871652	406.499649	6.648819
5.751876	403.403365	6.653824
6.169849	412.301063	6.658829
6.072320	430.487653	6.663834
5.820648	428.374167	6.668838
6.071765	420.250452	6.673843
5.923790	437.500462	6.678848
6.292138	440.383440	6.683853
5.958774	442.472972	6.688858
5.937182	440.237407	6.693862
6.449568	436.208134	6.698867
6.025788	412.879743	6.703872
5.912538	412.365085	6.708877
5.732171	415.710275	6.713882
6.388925	430.485697	6.718886
6.189665	415.779121	6.723891
5.876662	424.106148	6.728896
6.552225	415.180070	6.733901
6.277061	418.606829	6.738906
5.688488	406.462759	6.743910
6.004263	404.597540	6.748915
5.561521	417.355221	6.753920
6.017271	401.945814	6.758925
6.107760	410.844357	6.763930
6.208597	428.042880	6.768934
6.081975	411.021087	6.773939
5.931419	406.603956	6.778944
5.766717	413.709678	6.783949
5.783214	409.392009	6.788954
5.616420	432.775390	6.793958
5.958248	433.956498	6.798963
5.496654	439.151695	6.803968
5.934574	439.885797	6.808973
6.161750	444.379577	6.813978
6.033090	439.077722	6.818982
6.662173	444.306860	6.823987
6.352375	440.104370	6.828992
6.156049	430.223047	6.833997
6.218958	416.968076	6.839002
6.309557	403.641059	6.844006
6.245675	405.374597	6.849011
5.729517	408.836838	6.854016
6.007882	404.826516	6.859021
5.860912	406.806020	6.864026
5.759517	414.225167	6.869030
6.003372	419.662785	6.874035
6.120346	426.477594	6.879040
6.146030	418.470848	6.884045
5.823869	411.899613	6.889050
6.107462	430.661523	6.894054
6.078334	414.266653	6.899059
5.997193	419.451159	6.904064
6.229679	417.816943	6.909069
5.925238	416.687785	6.914074
5.604145	414.574032	6.919078
6.225514	417.101862	6.924083
6.214185	442.156444	6.929088
5.972917	426.197656	6.934093
5.932293	421.785340	6.939098
5.973428	428.413201	6.944102
5.946107	454.678092	6.949107
5.980465	446.957184	6.954112
6.071576	441.485036	6.959117
5.905166	452.137737	6.964122
6.091150	449.027022	6.969126
6.587654	437.091920	6.974131
6.352416	434.695041	6.979136
5.920680	415.109286	6.984141
5.972414	416.867028	6.989146
5.854776	416.285615	6.994150
6.121159	409.331018	6.999155
5.992962	411.639890	7.004160
5.993935	404.306614	7.009165
6.166188	400.260161	7.014170
6.108060	414.375610	7.019174
6.121008	410.639904	7.024179
5.845652	414.038281	7.029184
6.092672	408.286143	7.034189
5.997416	411.519499	7.039194
5.990157	402.911572	7.044198
5.935995	414.534917	7.049203
5.933100	412.743373	7.054208
5.963493	407.513013	7.059213
5.702368	411.730247	7.064218
6.150299	427.349941	7.069222
6.366681	419.104504	7.074227
6.101871	420.591460	7.079232
6.082175	415.162395	7.084237
6.108454	405.295109	7.089242
6.167387	412.771223	7.094246
6.340832	403.401210	7.099251
5.882297	406.836072	7.104256
5.785949	407.567109	7.109261
6.192323	413.898028	7.114266
6.111993	412.738444	7.119270
5.836806	417.479892	7.124275
5.995614	420.056047	7.129280
5.490635	406.582194	7.134285
5.992676	411.192336	7.139290
5.504980	427.162284	7.144294
6.121657	435.839614	7.149299
6.035677	437.805294	7.154304
6.408070	434.239556	7.159309
5.907905	425.299113	7.164314
5.787694	441.085520	7.169318
5.857380	438.663011	7.174323
5.632161	445.065664	7.179328
5.587138	440.923204	7.184333
5.885507	445.928983	7.189338
5.894071	445.957815	7.194342
6.106456	445.366356	7.199347
6.021370	448.214761	7.204352
6.376486	445.890501	7.209357
6.452796	449.097781	7.214362
6.305347	443.488363	7.219366
6.234879	442.092938	7.224371
6.125214	444.137314	7.229376
6.233769	432.378696	7.234381
6.149940	431.084037	7.239386
6.107589	422.255484	7.244390
6.149608	410.279293	7.249395
6.182988	414.270179	7.254400
5.979924	414.598678	7.259405
5.941487	409.750933	7.264410
5.549586	412.295269	7.269414
6.044138	414.824423	7.274419
6.248013	440.555240	7.279424
6.198199	424.171769	7.284429
5.907989	416.506881	7.289434
5.979773	426.891419	7.294438
5.866713	412.659341	7.299443
5.977449	414.539630	7.304448
6.293137	428.152226	7.309453
6.013045	415.707275	7.314458
6.103357	411.447847	7.319462
6.004853	413.206936	7.324467
5.939256	415.939647	7.329472
5.716468	409.707250	7.334477
5.949843	425.587828	7.339482
6.236049	444.866180	7.344486
5.928304	424.766446	7.349491
6.050822	454.513196	7.354496
6.430019	435.843002	7.359501
5.834402	424.460127	7.364506
5.586967	414.968269	7.369510
6.171848	431.859008	7.374515
6.191293	441.937395	7.379520
5.835563	423.246407	7.384525
5.674854	427.499536	7.389530
6.143769	432.426516	7.394534
6.544979	433.474885	7.399539
5.964888	432.456885	7.404544
6.090387	427.634725	7.409549
5.951146	409.910616	7.414554
5.838913	417.764457	7.419558
6.187232	422.859939	7.424563
5.907093	429.029955	7.429568
5.768239	437.254908	7.434573
6.329819	446.609448	7.439578
6.016754	448.635742	7.444582
6.594699	444.385890	7.449587
6.480037	423.309323	7.454592
6.288438	420.013979	7.459597
6.052894	415.844014	7.464602
5.855216	421.119996	7.469606
5.861517	410.190230	7.474611
5.659273	427.180953	7.479616
6.052762	411.472540	7.484621
5.900805	409.498157	7.489626
5.776530	420.891092	7.494630
5.787887	415.730072	7.499635
5.952805	417.361279	7.504640
5.804158	433.710670	7.509645
6.365034	441.253212	7.514650
6.120014	441.849589	7.519654
5.873153	428.290935	7.524659
5.649477	441.627454	7.529664
5.940242	433.536346	7.534669
5.845927	444.933226	7.539674
5.865196	443.128841	7.544678
6.429336	442.531046	7.549683
6.010679	446.289133	7.554688
6.563823	450.522954	7.559693
6.264698	443.256715	7.564698
6.125321	434.051539	7.569702
5.868515	413.500732	7.574707
5.912473	419.047645	7.579712
5.769513	412.073581	7.584717
5.726470	428.911224	7.589722
5.894568	441.709057	7.594726
6.339433	441.514152	7.599731
5.886190	446.522598	7.604736
6.352357	446.663155	7.609741
6.496135	455.067925	7.614746
6.180394	432.375837	7.619750
6.110386	412.698935	7.624755
6.007156	422.577678	7.629760
6.199669	409.253546	7.634765
6.328022	411.298243	7.639770
5.830915	420.103490	7.644774
6.205622	408.875873	7.649779
5.864837	410.061066	7.654784
6.123045	419.328592	7.659789
6.190273	416.794914	7.664794
5.869920	416.436716	7.669798
5.785547	412.450032	7.674803
6.005430	419.360200	7.679808
5.976758	407.070624	7.684813
5.937838	411.905026	7.689818
5.909902	416.403369	7.694822
6.064384	410.828713	7.699827
5.629060	417.141178	7.704832
5.653703	410.072825	7.709837
6.449472	426.185139	7.714842
5.857337	437.982349	7.719846
6.174712	420.585481	7.724851
6.052500	418.620586	7.729856
5.987505	416.606378	7.734861
5.864957	415.791765	7.739866
5.881696	434.764803	7.744870
6.091578	436.366581	7.749875
5.738193	437.142760	7.754880
5.979759	450.523749	7.759885
6.184921	452.563255	7.764890
5.906887	451.387506	7.769894
6.122241	453.650856	7.774899
6.200170	442.255512	7.779904
6.090848	450.815265	7.784909
6.420344	443.826446	7.789914
5.788017	436.912920	7.794918
5.795839	417.284119	7.799923
5.749766	434.875998	7.804928
5.901183	444.495039	7.809933
6.249437	441.695109	7.814938
6.061227	461.081184	7.819942
6.187282	448.701779	7.824947
5.917372	454.079683	7.829952
6.143336	448.899860	7.834957
6.335107	449.488279	7.839962
5.886666	435.072661	7.844966
6.163413	419.767106	7.849971
5.687895	416.964014	7.854976
6.123339	433.601241	7.859981
6.419053	437.194409	7.864986
6.310033	428.031476	7.869990
6.426530	412.231311	7.874995
6.050656	418.944853	7.880000
5.803761	402.560333	7.885005
6.016020	411.750406	7.890010
5.793559	426.762970	7.895014
6.250694	410.534681	7.900019
5.931551	419.212849	7.905024
6.009155	409.588749	7.910029
5.922287	410.663021	7.915034
5.764004	414.436278	7.920038
6.057571	412.011602	7.925043
5.807601	422.664674	7.930048
6.086039	411.192611	7.935053
5.943037	409.717130	7.940058
5.729031	414.156347	7.945062
6.187126	440.592765	7.950067
5.916762	444.100620	7.955072
6.309560	443.826714	7.960077
5.669908	431.387798	7.965082
6.001744	444.512156	7.970086
6.135437	436.225423	7.975091
6.318547	453.774122	7.980096
6.248712	442.787659	7.985101
6.180148	429.874937	7.990106
5.667114	419.333665	7.995110
6.216466	414.923791	8.000115
5.967910	428.586242	8.005133
5.988047	423.486822	8.010150
6.019038	415.015861	8.015168
5.799979	419.958153	8.020186
6.206548	414.523673	8.025203
6.061872	419.970195	8.030221
5.814371	430.695675	8.035238
6.023852	422.207416	8.040256
6.015763	443.609940	8.045274
6.493465	444.564791	8.050291
6.301673	430.514121	8.055309
6.064659	417.057523	8.060326
6.199391	429.026837	8.065344
5.780244	422.384315	8.070362
6.029569	415.073178	8.075379
6.218398	418.423095	8.080397
6.022374	410.784856	8.085414
6.102495	408.236984	8.090432
5.848039	432.368801	8.095450
6.103754	432.914369	8.100467
6.065633	433.810497	8.105485
6.193879	446.040290	8.110502
6.338675	442.761602	8.115520
6.295981	437.191954	8.120538
5.907944	417.853112	8.125555
6.327237	438.743660	8.130573
6.017669	433.808443	8.135590
6.334973	417.253108	8.140608
5.978941	429.464218	8.145626
6.255792	434.658742	8.150643
6.134103	446.094485	8.155661
6.287289	447.963018	8.160678
6.515616	437.068605	8.165696
5.918403	421.509098	8.170714
6.194906	424.679209	8.175731
5.909138	443.000340	8.180749
6.371357	435.842061	8.185766
6.331954	436.128197	8.190784
6.200274	454.092157	8.195802
6.269614	444.598818	8.200819
6.394225	444.478994	8.205837
5.971807	440.559653	8.210854
6.278003	436.370034	8.215872
6.317725	451.662234	8.220890
6.305369	431.696253	8.225907
5.994690	437.056459	8.230925
6.332250	456.777917	8.235942
6.616171	451.261353	8.240960
6.243465	444.408040	8.245978
6.025650	444.276019	8.250995
6.065021	445.749768	8.256013
6.443781	436.849749	8.261030
6.475980	449.508813	8.266048
6.312186	455.540765	8.271066
6.474866	441.748269	8.276083
6.426358	427.128862	8.281101
6.207354	427.522516	8.286118
6.257837	429.699689	8.291136
6.202042	433.456296	8.296154
6.437757	436.242190	8.301171
5.928900	438.923326	8.306189
6.297367	441.154424	8.311206
6.487061	433.945141	8.316224
6.125246	452.686244	8.321242
6.318340	439.369723	8.326259
6.293840	447.370058	8.331277
6.193015	453.663002	8.336294
6.177026	445.899148	8.341312
6.248564	446.787881	8.346330
6.323808	443.336573	8.351347
5.991054	451.211216	8.356365
6.153018	444.561018	8.361382
6.336903	446.472990	8.366400
6.146853	452.425341	8.371418
6.414773	437.987145	8.376435
6.212815	443.485160	8.381453
5.970427	440.723413	8.386470
6.572635	455.848170	8.391488
6.378841	477.676721	8.396506
6.514236	472.060213	8.401523
6.562723	470.564286	8.406541
6.303276	480.254395	8.411558
6.479772	478.374003	8.416576
6.316585	479.658638	8.421594
6.764711	481.419589	8.426611
6.728755	484.774785	8.431629
6.533605	459.547572	8.436646
6.749049	457.331584	8.441664
6.744629	454.043505	8.446682
6.743395	440.185499	8.451699
6.800378	452.605284	8.456717
6.273844	454.642631	8.461734
6.552364	452.843983	8.466752
6.456561	448.975071	8.471770
6.221449	453.046196	8.476787
6.572621	453.101386	8.481805
6.679452	462.380733	8.486822
6.722532	439.102837	8.491840
6.943889	446.743417	8.496858
6.474084	447.333112	8.501875
6.825600	438.257614	8.506893
6.578241	443.981195	8.511910
6.425521	439.612253	8.516928
6.041714	444.796791	8.521946
6.552229	448.651014	8.526963
6.835230	448.673877	8.531981
6.343015	446.865326	8.536998
6.460299	446.048141	8.542016
6.452315	448.478332	8.547034
6.564588	446.005832	8.552051
6.653798	446.905914	8.557069
6.221643	456.143451	8.562087
6.542764	450.069970	8.567104
6.417144	462.359540	8.572122
6.618056	479.928973	8.577139
6.945041	474.856467	8.582157
6.204967	472.296817	8.587175
6.699421	470.192461	8.592192
6.273089	474.115900	8.597210
6.738159	483.687165	8.602227
6.680891	478.513331	8.607245
6.899896	487.166705	8.612263
6.949607	477.119621	8.617280
7.037277	481.949150	8.622298
6.525817	463.377242	8.627315
6.563696	456.589311	8.632333
6.454265	472.731694	8.637351
6.944736	473.792091	8.642368
6.871730	471.418203	8.647386
6.720318	480.691921	8.652403
6.692976	466.213339	8.657421
6.594167	475.827893	8.662439
6.961995	475.521056	8.667456
6.764833	473.113760	8.672474
6.417401	465.277629	8.677491
7.112379	470.591314	8.682509
6.756549	470.694360	8.687527
6.724654	456.416890	8.692544
6.804783	460.871262	8.697562
6.466184	464.843769	8.702579
6.936219	467.211598	8.707597
6.507223	480.909987	8.712615
6.582461	483.210117	8.717632
6.667107	476.356094	8.722650
6.292203	481.124596	8.727667
6.811769	473.180805	8.732685
6.458286	485.673074	8.737703
6.913882	476.753742	8.742720
7.035102	483.047102	8.747738
6.937219	475.313888	8.752755
7.240178	476.988221	8.757773
6.622966	480.885344	8.762791
6.875517	478.252776	8.767808
6.717685	481.948223	8.772826
6.709221	491.801150	8.777843
6.853852	472.509419	8.782861
6.814297	478.766958	8.787879
6.936994	490.475766	8.792896
6.650479	484.095688	8.797914
6.433792	479.063628	8.802931
6.877928	478.897297	8.807949
7.000227	487.384211	8.812967
6.739908	479.260506	8.817984
7.086462	492.053836	8.823002
6.857875	481.134528	8.828019
6.992183	468.873047	8.833037
6.718351	482.181207	8.838055
6.582252	479.096735	8.843072
6.549955	491.577654	8.848090
6.905990	503.716611	8.853107
7.285913	506.452217	8.858125
7.142962	515.341665	8.863143
6.929590	500.184788	8.868160
6.934289	493.283352	8.873178
7.136371	504.936148	8.878195
7.153320	498.607664	8.883213
7.128742	489.188664	8.888231
6.756945	484.145334	8.893248
6.835637	492.372092	8.898266
6.869635	509.322231	8.903283
6.611181	518.782130	8.908301
6.851666	525.823355	8.913319
6.825903	515.328184	8.918336
6.920227	518.366841	8.923354
6.521721	524.774054	8.928371
7.040546	524.649306	8.933389
6.630650	517.062299	8.938407
6.919046	522.622979	8.943424
7.065077	517.474775	8.948442
7.057248	521.264216	8.953459
6.796671	513.530612	8.958477
6.994974	524.531624	8.963495
7.280461	545.343958	8.968512
6.849908	528.236150	8.973530
7.151911	531.357886	8.978547
7.358148	538.628942	8.983565
7.080464	534.811616	8.988583
7.042530	511.824992	8.993600
7.281405	527.365695	8.998618
6.903270	523.314925	9.003635
6.950215	522.561613	9.008653
6.924136	534.867658	9.013671
7.383822	551.005326	9.018688
7.522831	544.696506	9.023706
7.128905	541.929769	9.028723
7.148662	525.607408	9.033741
6.912124	525.139673	9.038759
7.252898	539.676156	9.043776
7.332363	537.164978	9.048794
7.084407	532.951482	9.053811
7.280252	538.428663	9.058829
7.287203	540.551838	9.063847
7.288734	541.320185	9.068864
7.252672	520.919219	9.073882
7.089923	518.030934	9.078899
7.526187	518.952095	9.083917
7.320906	527.250992	9.088935
7.224016	506.532606	9.093952
7.358722	498.134009	9.098970
7.167241	515.500274	9.103987
7.264651	511.630413	9.109005
7.234603	503.802627	9.114023
7.132239	510.193662	9.119040
7.244455	513.547700	9.124058
7.096046	515.400742	9.129075
7.407738	525.847793	9.134093
7.610888	532.056585	9.139111
7.376058	521.985643	9.144128
7.278037	521.795054	9.149146
7.115217	524.118392	9.154163
7.271258	509.543335	9.159181
7.324848	514.028580	9.164199
7.371551	535.963994	9.169216
7.777387	534.197830	9.174234
7.077039	520.869766	9.179251
7.202166	515.185564	9.184269
7.150075	517.476924	9.189287
7.281496	536.695556	9.194304
7.679645	541.792824	9.199322
7.145287	538.141018	9.204339
7.517386	547.310549	9.209357
7.429806	550.752720	9.214375
7.332222	537.783204	9.219392
7.660821	544.299942	9.224410
7.178278	538.994540	9.229427
7.345916	530.765446	9.234445
7.175891	536.988774	9.239463
7.438263	554.556008	9.244480
7.284358	544.965276	9.249498
7.362465	548.657174	9.254515
7.275181	542.085616	9.259533
7.240112	544.097551	9.264551
7.206154	531.987227	9.269568
7.215819	535.738454	9.274586
7.191177	542.360505	9.279603
7.210005	540.201304	9.284621
7.451181	554.167964	9.289639
7.302278	543.694896	9.294656
7.611535	538.698414	9.299674
7.299723	550.553861	9.304691
7.424593	547.491097	9.309709
7.763687	562.342676	9.314727
7.590579	571.322064	9.319744
7.929228	558.785650	9.324762
7.765557	549.321111	9.329779
7.649479	545.557865	9.334797
7.368847	539.509006	9.339815
7.360134	546.870498	9.344832
7.707576	550.029405	9.349850
7.388134	552.717635	9.354867
7.305092	540.674262	9.359885
7.572914	544.882528	9.364903
7.467438	560.135065	9.369920
7.796536	561.748505	9.374938
7.662617	568.434385	9.379955
7.602951	547.123988	9.384973
7.602764	544.117612	9.389991
7.611265	545.167230	9.395008
7.594152	544.527336	9.400026
7.441870	564.367276	9.405043
7.888851	574.243887	9.410061
7.833817	557.393904	9.415079
7.631933	548.108971	9.420096
7.451970	543.240077	9.425114
7.692028	564.960547	9.430131
7.657321	567.379133	9.435149
7.944441	575.834233	9.440167
7.804235	566.213474	9.445184
7.753470	541.301566	9.450202
7.454079	546.455754	9.455219
7.537733	544.295877	9.460237
7.492836	556.732484	9.465255
7.561770	575.918981	9.470272
7.747711	568.020829	9.475290
7.864894	567.039318	9.480307
7.862038	571.584881	9.485325
7.713022	574.675867	9.490343
8.113180	578.324292	9.495360
8.075216	564.630873	9.500378
7.634195	548.710749	9.505395
7.620682	546.124599	9.510413
8.033355	552.495288	9.515431
7.427392	559.114124	9.520448
7.839054	561.276993	9.525466
7.782452	572.633683	9.530483
7.585982	569.495993	9.535501
7.905201	567.264218	9.540519
7.868307	578.098372	9.545536
8.102062	580.668913	9.550554
7.782896	582.938881	9.555571
7.901128	577.497576	9.560589
7.932060	584.104558	9.565607
8.009953	587.801912	9.570624
8.020746	566.246428	9.575642
7.710494	568.084694	9.580659
7.928544	578.506025	9.585677
7.676059	570.947101	9.590695
7.811538	578.597806	9.595712
8.086144	566.470314	9.600730
7.861673	575.142804	9.605747
7.688206	585.623625	9.610765
7.658780	574.620167	9.615783
7.675084	578.837042	9.620800
7.745280	576.976272	9.625818
7.709472	571.496560	9.630835
7.930602	575.656460	9.635853
8.169988	577.986355	9.640871
7.889844	577.256786	9.645888
7.989186	566.633644	9.650906
7.981985	567.557341	9.655923
8.094674	578.169670	9.660941
8.192697	577.835682	9.665959
7.960702	586.109109	9.670976
7.823572	579.801528	9.675994
7.806051	575.633682	9.681011
7.793793	574.653979	9.686029
8.039582	572.384053	9.691047
8.008978	582.936421	9.696064
8.175051	571.021801	9.701082
8.034137	590.218689	9.706099
7.777747	582.836747	9.711117
7.922624	567.637820	9.716135
7.704341	583.836982	9.721152
8.037578	583.326946	9.726170
8.168247	581.045439	9.731187
8.079293	593.904429	9.736205
8.017992	579.534677	9.741223
8.126553	591.935226	9.746240
7.967214	592.491135	9.751258
8.254211	592.203066	9.756275
8.107808	600.264562	9.761293
8.515589	588.856823	9.766311
8.007429	591.747078	9.771328
7.880252	579.925294	9.776346
7.966706	589.148845	9.781363
8.050297	598.563486	9.786381
8.030503	604.217440	9.791399
7.912485	603.393965	9.796416
7.996597	590.015222	9.801434
8.190328	607.308092	9.806451
7.942851	602.684639	9.811469
8.121776	599.997499	9.816487
7.764720	611.521267	9.821504
8.395005	600.378755	9.826522
8.175435	604.495865	9.831539
8.219565	604.818288	9.836557
8.380226	602.379688	9.841575
8.195277	599.960414	9.846592
8.121613	600.496556	9.851610
7.980905	610.133764	9.856627
8.012756	604.186653	9.861645
8.250899	600.747948	9.866663
8.308965	620.135567	9.871680
8.192326	627.426073	9.876698
8.382928	623.311401	9.881715
8.547565	628.877614	9.886733
8.537761	612.380259	9.891751
8.172365	616.768076	9.896768
8.294255	597.175186	9.901786
8.096727	606.481202	9.906803
8.430349	620.376652	9.911821
8.152844	621.706957	9.916839
8.426531	636.164183	9.921856
8.233241	637.454692	9.926874
8.601451	637.532653	9.931891
8.227716	635.739629	9.936909
8.793448	629.289010	9.941927
8.443166	623.212364	9.946944
8.554810	609.258698	9.951962
8.445937	596.809298	9.956979
8.299693	606.224236	9.961997
8.768610	596.261408	9.967015
8.306467	596.078148	9.972032
8.676830	596.399797	9.977050
8.505479	591.874375	9.982067
8.255654	596.548339	9.987085
8.256435	592.713714	9.992103
8.200159	606.764906	9.997120
8.501218	619.612308	10.002138
8.975340	618.028610	10.007155
8.501584	615.668378	10.012173
8.626306	596.567245	10.017191
8.443187	596.798213	10.022208
8.318778	604.060963	10.027226
8.682486	591.506310	10.032243
8.109583	603.837829	10.037261
8.626885	614.002489	10.042279
8.891726	626.238783	10.047296
8.742626	621.802570	10.052314
8.566521	597.691441	10.057331
8.549721	606.782196	10.062349
8.452992	602.401789	10.067367
8.546207	606.164613	10.072384
8.560808	605.945472	10.077402
8.623022	609.801789	10.082419
8.380535	609.417007	10.087437
8.877234	598.180158	10.092455
8.845970	614.196803	10.097472
8.587788	608.571482	10.102490
8.573179	601.586297	10.107507
8.548968	615.845344	10.112525
8.762886	607.655008	10.117543
8.391576	602.187234	10.122560
8.317183	605.422359	10.127578
8.831838	616.089324	10.132595
8.845996	632.804934	10.137613
9.132199	623.517626	10.142631
8.837874	611.106341	10.147648
8.315873	606.265315	10.152666
8.677174	601.502880	10.157683
8.508900	609.217574	10.162701
8.956492	620.405267	10.167719
8.650986	619.833005	10.172736
8.541364	623.826264	10.177754
8.818157	641.233371	10.182771
8.656066	635.113517	10.187789
9.008397	633.419261	10.192807
8.825558	644.705152	10.197824
8.704517	638.574773	10.202842
8.987348	630.569848	10.207859
8.685719	622.209143	10.212877
9.050787	615.567326	10.217895
8.700555	619.619830	10.222912
8.724030	608.506150	10.227930
8.837048	613.197503	10.232947
8.618288	643.511871	10.237965
9.092928	631.576816	10.242983
8.665888	636.564274	10.248000
8.851568	642.775604	10.253018
8.833592	625.585532	10.258035
8.710318	637.506228	10.263053
8.644296	633.478539	10.268071
8.610031	639.373629	10.273088
8.633841	634.448202	10.278106
8.723561	635.215953	10.283123
8.734825	646.431390	10.288141
9.059195	630.338247	10.293159
8.701082	631.024230	10.298176
8.592628	639.306497	10.303194
8.886418	635.424916	10.308211
8.615216	646.975459	10.313229
8.892591	648.512236	10.318247
9.109812	658.916046	10.323264
9.065848	660.691128	10.328282
9.021649	651.661514	10.333299
9.080070	664.453992	10.338317
9.180258	652.231462	10.343335
8.967912	645.719791	10.348352
8.770099	635.684381	10.353370
9.376182	635.705417	10.358387
9.079909	642.189760	10.363405
9.202465	625.415156	10.368423
8.927645	631.923503	10.373440
8.916876	634.426119	10.378458
8.961434	631.550197	10.383475
8.707023	639.025944	10.388493
9.100860	648.747935	10.393511
9.421122	657.696224	10.398528
9.122307	661.015583	10.403546
9.328424	657.949506	10.408563
8.731468	645.812274	10.413581
9.210809	647.164131	10.418599
8.816356	662.091075	10.423616
9.221366	664.132543	10.428634
9.145922	654.608485	10.433651
9.001917	664.137141	10.438669
9.033546	665.543109	10.443687
9.440499	662.727742	10.448704
9.170553	675.245033	10.453722
9.575410	661.893325	10.458739
8.812179	669.847090	10.463757
9.011927	680.574900	10.468775
9.690523	658.426542	10.473792
9.417887	668.959825	10.478810
9.308720	666.522900	10.483827
8.920286	665.951450	10.488845
9.001739	659.792617	10.493863
9.468041	667.826404	10.498880
9.362850	667.656481	10.503898
9.293651	664.933578	10.508915
9.388442	675.558182	10.513933
9.382086	665.315754	10.518951
9.117507	664.916613	10.523968
8.907076	674.319271	10.528986
9.289573	668.377168	10.534003
9.121406	679.435310	10.539021
8.972011	666.835593	10.544039
9.125012	656.869039	10.549056
8.937439	669.268501	10.554074
9.206251	658.587276	10.559091
9.292008	666.634648	10.564109
8.852410	671.514371	10.569127
9.612303	667.460006	10.574144
9.401161	696.116069	10.579162
9.675063	690.479051	10.584179
9.362670	675.466194	10.589197
9.340235	671.090022	10.594215
9.297467	666.269367	10.599232
9.271053	694.071833	10.604250
9.647750	688.946661	10.609267
9.430281	699.125837	10.614285
9.709326	699.409047	10.619303
9.575520	677.220051	10.624320
9.288000	675.863473	10.629338
9.449510	680.112077	10.634355
9.628909	686.912438	10.639373
9.318854	690.361096	10.644391
9.605851	677.639558	10.649408
9.702628	687.167603	10.654426
9.547683	679.787546	10.659443
9.563219	676.237314	10.664461
9.510564	671.728762	10.669479
9.632336	665.708511	10.674496
9.222611	669.014022	10.679514
9.192233	691.342242	10.684531
9.501670	697.556760	10.689549
9.521727	695.130162	10.694567
9.764380	696.978627	10.699584
9.541864	706.831541	10.704602
9.842031	696.479295	10.709619
9.922341	696.198418	10.714637
9.315894	705.454180	10.719655
9.977020	698.934431	10.724672
9.707910	703.167706	10.729690
10.054587	694.735448	10.734707
9.630221	687.376687	10.739725
9.606033	673.856844	10.744743
9.601419	659.380523	10.749760
9.491896	674.703218	10.754778
9.873302	687.636396	10.759795
9.637832	690.647714	10.764813
9.713704	698.366684	10.769831
9.902185	693.002885	10.774848
9.966679	691.810727	10.779866
9.890213	682.558913	10.784883
9.525347	675.296604	10.789901
9.288608	668.750379	10.794919
9.612998	686.114738	10.799936
9.824877	700.149549	10.804954
10.037023	698.153813	10.809971
10.160326	704.802263	10.814989
10.047450	686.618161	10.820007
9.996884	663.316728	10.825024
9.599294	665.773847	10.830042
9.522853	664.455798	10.835059
9.621805	664.630313	10.840077
9.860633	694.597169	10.845095
9.995512	702.202768	10.850112
9.739055	697.150541	10.855130
9.926307	698.113061	10.860147
9.919694	699.741157	10.865165
9.559340	699.035365	10.870183
10.236243	694.125982	10.875200
9.586460	706.535236	10.880218
9.826056	709.827231	10.885235
9.734931	705.245809	10.890253
9.864032	707.256221	10.895271
9.846083	693.212204	10.900288
9.932885	700.953183	10.905306
9.957060	703.448460	10.910323
9.604455	704.715509	10.915341
9.529442	704.742134	10.920359
10.113360	700.082419	10.925376
9.730100	693.583327	10.930394
9.892510	694.236136	10.935411
9.885596	704.929526	10.940429
9.610042	706.489195	10.945447
10.270563	704.714283	10.950464
10.150245	713.431634	10.955482
9.988989	714.018370	10.960499
10.307564	702.883210	10.965517
10.099053	707.778682	10.970535
10.225255	700.469946	10.975552
9.999929	699.910016	10.980570
9.907960	692.143734	10.985587
9.893485	705.683385	10.990605
10.065949	717.252474	10.995623
10.328504	712.545686	11.000640
10.268029	717.651395	11.005658
10.001420	712.992299	11.010675
10.379590	711.376918	11.015693
10.142360	704.936546	11.020711
10.146146	711.216834	11.025728
9.876082	721.040909	11.030746
10.339736	705.666257	11.035763
10.260983	723.158489	11.040781
9.886222	730.569343	11.045799
10.177680	718.743907	11.050816
10.057145	723.963165	11.055834
9.877822	721.945915	11.060851
10.087946	715.361151	11.065869
10.035677	722.065980	11.070887
10.502655	724.934158	11.075904
10.100285	725.384003	11.080922
10.392872	731.300394	11.085939
10.523861	719.608049	11.090957
10.322098	724.166552	11.095975
10.093960	727.867771	11.100992
9.924086	729.712183	11.106010
9.972595	725.952003	11.111027
10.479053	728.000037	11.116045
10.417350	734.647092	11.121063
10.684809	728.569676	11.126080
10.216014	730.165710	11.131098
10.330919	735.507843	11.136115
10.562107	716.779737	11.141133
10.057289	730.224295	11.146151
10.378592	728.986250	11.151168
10.403270	726.892874	11.156186
10.293333	713.821924	11.161203
10.402268	724.701851	11.166221
10.389643	728.423449	11.171239
10.394163	725.938402	11.176256
10.291622	727.493197	11.181274
10.601051	740.420798	11.186291
10.780779	723.126797	11.191309
10.242515	730.799960	11.196327
10.395743	727.505746	11.201344
10.178419	733.318646	11.206362
10.532846	753.327799	11.211379
11.068384	742.250833	11.216397
10.853310	738.275204	11.221415
10.543609	720.773758	11.226432
10.517977	726.980583	11.231450
10.551627	724.687337	11.236467
10.728792	717.335532	11.241485
10.306572	728.406959	11.246503
10.494634	732.289449	11.251520
10.712386	726.902202	11.256538
10.435782	729.732666	11.261555
10.553002	724.870595	11.266573
10.623417	750.425117	11.271591
10.969655	753.184539	11.276608
10.735294	736.017605	11.281626
10.603937	728.932289	11.286643
10.815993	730.263868	11.291661
10.765728	733.931561	11.296679
10.534172	727.502936	11.301696
10.487818	722.055616	11.306714
10.520508	734.292179	11.311731
10.658312	747.991312	11.316749
10.828892	752.210489	11.321767
10.894962	756.284766	11.326784
10.755090	754.766504	11.331802
10.935266	757.202552	11.336819
10.921072	734.281737	11.341837
10.491790	738.830608	11.346855
10.556752	749.049052	11.351872
10.944705	746.007425	11.356890
10.901275	750.160807	11.361907
10.760002	759.055728	11.366925
10.722633	759.129174	11.371943
11.037162	756.359176	11.376960
10.848239	760.276812	11.381978
10.614496	756.843432	11.386995
10.529792	752.417696	11.392013
10.718296	758.819712	11.397031
10.807616	757.005849	11.402048
10.769277	751.852609	11.407066
11.012935	757.283196	11.412083
11.044611	757.022951	11.417101
10.662690	759.334903	11.422119
11.005905	761.573372	11.427136
10.881311	754.445498	11.432154
10.598932	757.094869	11.437171
10.846306	759.445810	11.442189
10.399703	760.263427	11.447207
10.499188	752.614463	11.452224
10.796579	770.389009	11.457242
10.838196	779.941381	11.462259
11.320228	785.517195	11.467277
11.218435	790.082716	11.472295
11.128392	789.282160	11.477312
11.325052	786.517072	11.482330
11.012596	778.609264	11.487347
11.549800	758.312913	11.492365
10.830750	766.283241	11.497383
10.847753	760.829374	11.502400
11.026533	755.177547	11.507418
11.005468	769.453338	11.512435
11.071942	771.001856	11.517453
11.090031	789.416365	11.522471
11.092029	787.882528	11.527488
11.405437	788.405979	11.532506
11.028458	795.984522	11.537523
11.119018	789.421354	11.542541
10.939146	790.149037	11.547559
11.277678	800.440491	11.552576
11.543120	790.406558	11.557594
11.460171	799.586394	11.562611
11.218675	788.444141	11.567629
11.037283	781.908206	11.572647
11.326623	786.369233	11.577664
11.258571	797.852269	11.582682
11.404325	800.463960	11.587699
11.433320	783.857371	11.592717
11.248427	779.117539	11.597735
11.239260	777.916587	11.602752
11.403203	767.957010	11.607770
10.968452	773.776039	11.612787
11.368525	779.479645	11.617805
11.275432	779.792570	11.622823
11.369200	789.416629	11.627840
11.479620	786.567189	11.632858
11.225688	792.673508	11.637875
11.498558	790.519032	11.642893
11.406485	793.751804	11.647911
11.021347	794.238066	11.652928
11.389999	788.232371	11.657946
10.974908	788.819727	11.662963
11.398652	791.822598	11.667981
11.003062	800.492298	11.672999
11.078292	790.688088	11.678016
11.289691	793.335180	11.683034
11.325279	802.454984	11.688051
11.298456	794.522304	11.693069
11.415987	798.119672	11.698087
11.226959	816.864842	11.703104
11.711173	822.324780	11.708122
11.497871	820.127832	11.713139
11.594200	824.915691	11.718157
11.731661	818.726087	11.723175
11.767079	811.202718	11.728192
11.468877	801.150036	11.733210
11.288687	806.505042	11.738227
11.586107	813.075759	11.743245
11.241239	814.732900	11.748263
11.366555	816.420588	11.753280
11.685827	815.394348	11.758298
11.787911	826.132495	11.763315
11.717015	819.919656	11.768333
11.777321	821.247193	11.773351
11.695306	822.314150	11.778368
11.948543	821.206517	11.783386
11.600388	820.509234	11.788403
11.647870	824.683629	11.793421
11.730017	823.533811	11.798439
11.411760	822.182299	11.803456
12.023411	826.536737	11.808474
11.728425	825.962729	11.813491
11.528534	829.594552	11.818509
11.424219	830.009806	11.823527
11.373537	829.525322	11.828544
11.522084	812.597132	11.833562
11.493849	824.981310	11.838579
11.703902	833.175127	11.843597
11.613581	824.185999	11.848615
11.367230	817.211460	11.853632
11.398940	835.397044	11.858650
12.265822	840.507189	11.863667
12.291998	851.770794	11.868685
12.047486	835.630825	11.873703
11.614066	824.760867	11.878720
11.649087	835.059203	11.883738
11.813564	835.134424	11.888755
12.010887	839.017674	11.893773
12.095457	843.764577	11.898791
11.902314	844.825987	11.903808
12.035735	825.941890	11.908826
11.805386	833.309050	11.913843
11.924462	832.333310	11.918861
12.226968	838.534468	11.923879
11.759195	840.807382	11.928896
12.175362	841.900062	11.933914
12.105429	843.157114	11.938931
11.907136	830.017415	11.943949
12.136527	829.960966	11.948967
11.712883	829.472281	11.953984
11.720389	847.018792	11.959002
12.091149	849.302023	11.964019
12.139285	856.951654	11.969037
12.198836	859.103772	11.974055
12.541819	863.931871	11.979072
12.494746	851.919409	11.984090
12.081489	837.923563	11.989107
12.090847	830.020902	11.994125
11.996727	823.598358	11.999143
11.760794	824.436566	12.004160
12.026565	845.476244	12.009178
12.183299	857.921498	12.014195
12.276152	848.523022	12.019213
12.405831	849.661374	12.024231
12.146449	849.991252	12.029248
12.440835	844.896656	12.034266
12.352232	856.582897	12.039283
12.203204	865.746335	12.044301
12.392308	849.555458	12.049319
12.246728	844.883898	12.054336
12.369405	841.642436	12.059354
12.283634	830.222497	12.064371
12.311067	834.797476	12.069389
12.370470	835.898533	12.074407
12.143962	829.153735	12.079424
12.298832	838.044635	12.084442
12.292089	853.581976	12.089459
12.365631	857.498774	12.094477
12.316954	850.147916	12.099495
12.550401	852.238525	12.104512
12.445408	859.100131	12.109530
12.208813	867.637708	12.114547
12.038503	858.340973	12.119565
12.506987	852.239636	12.124583
12.364912	856.925886	12.129600
12.466867	848.406156	12.134618
12.187140	855.326748	12.139635
12.341896	858.649230	12.144653
12.251957	857.371676	12.149671
12.001947	854.664843	12.154688
12.379708	852.400424	12.159706
12.322112	849.636011	12.164723
12.547000	850.024613	12.169741
12.597995	855.255129	12.174759
12.197092	865.911791	12.179776
12.163216	853.676322	12.184794
12.475950	864.471202	12.189811
12.649737	875.315228	12.194829
12.906358	882.795897	12.199847
12.957009	883.763290	12.204864
12.679461	858.041161	12.209882
12.477420	858.551192	12.214899
12.487516	850.808409	12.219917
12.731620	847.593819	12.224935
12.677229	854.323363	12.229952
12.437294	858.991638	12.234970
12.528303	872.160231	12.239987
12.602762	879.789385	12.245005
13.139050	875.876230	12.250023
12.858360	875.961250	12.255040
12.939076	859.440209	12.260058
12.838717	852.902366	12.265075
12.582676	845.299807	12.270093
12.753037	851.768333	12.275111
12.239199	869.302125	12.280128
12.350593	863.702233	12.285146
12.809664	873.138835	12.290163
12.816260	877.077034	12.295181
13.173087	874.642974	12.300199
12.954961	879.432038	12.305216
12.939652	889.133820	12.310234
12.810996	878.271126	12.315251
12.984670	878.444514	12.320269
13.383482	879.049014	12.325287
12.998004	880.682466	12.330304
13.064577	864.224277	12.335322
12.906728	855.816755	12.340339
12.546364	851.291100	12.345357
13.077122	870.427428	12.350375
13.086465	884.233820	12.355392
13.067490	880.354956	12.360410
13.057748	861.210176	12.365427
12.905275	862.516886	12.370445
13.090705	861.462574	12.375463
12.942385	867.957201	12.380480
13.422471	876.490007	12.385498
13.252754	855.449094	12.390515
13.104813	850.845035	12.395533
12.970443	846.408487	12.400551
12.833273	851.954296	12.405568
13.048463	848.860211	12.410586
12.939782	848.872719	12.415603
13.207980	871.022060	12.420621
13.297761	862.451981	12.425639
12.968368	860.110561	12.430656
13.231919	879.095228	12.435674
13.385437	875.047138	12.440691
13.522863	870.508197	12.445709
13.386934	858.228183	12.450727
12.970683	862.796980	12.455744
12.815049	857.093510	12.460762
12.826686	871.251119	12.465779
13.172298	872.734230	12.470797
13.486109	876.161509	12.475815
13.298494	880.325272	12.480832
13.723066	886.548100	12.485850
13.589481	863.380336	12.490867
13.340825	856.385592	12.495885
13.157937	852.750023	12.500903
12.986341	852.734549	12.505920
12.898559	858.712766	12.510938
13.168365	872.366873	12.515955
12.936660	878.595415	12.520973
13.064051	877.141320	12.525991
13.193189	885.477253	12.531008
12.985565	868.613963	12.536026
13.067945	880.188123	12.541043
13.067782	890.219724	12.546061
13.403145	881.402297	12.551079
13.204529	908.293328	12.556096
13.632086	911.905816	12.561114
13.545149	908.312044	12.566131
13.023098	923.934515	12.571149
13.534993	911.060679	12.576167
13.433769	897.223018	12.581184
13.586122	916.945660	12.586202
13.280032	909.909506	12.591219
13.448947	906.452161	12.596237
13.877351	907.187869	12.601255
13.348780	914.828916	12.606272
13.643582	911.658583	12.611290
13.863638	900.555602	12.616307
13.584508	907.842194	12.621325
13.737795	902.552039	12.626343
13.623961	899.527768	12.631360
13.652294	902.740073	12.636378
14.222261	900.742255	12.641395
13.604137	902.792038	12.646413
13.699660	905.933114	12.651431
13.717301	909.080566	12.656448
13.690794	913.743504	12.661466
14.211702	902.842923	12.666483
13.728478	905.238654	12.671501
14.044836	891.413273	12.676519
13.790968	879.239035	12.681536
13.442602	886.827852	12.686554
13.894043	888.058086	12.691571
13.765122	901.196131	12.696589
13.808421	898.953224	12.701607
14.032921	905.991558	12.706624
13.618451	892.552945	12.711642
13.927452	889.555041	12.716659
13.922123	902.312494	12.721677
14.174701	896.467448	12.726695
14.037948	890.537363	12.731712
13.821986	880.247261	12.736730
13.745884	851.305039	12.741747
13.706987	887.179180	12.746765
13.965384	900.261681	12.751783
14.055211	899.595440	12.756800
14.036170	917.182041	12.761818
14.465159	896.943148	12.766835
13.989250	886.340454	12.771853
13.751173	877.666702	12.776871
14.089391	886.210264	12.781888
13.995055	895.421069	12.786906
13.961745	886.792002	12.791923
14.062426	898.381356	12.796941
14.340825	895.830061	12.801959
14.194477	894.869545	12.806976
13.917530	865.681504	12.811994
14.487251	884.468955	12.817011
13.952296	887.748168	12.822029
13.990067	876.978815	12.827047
14.128109	888.089832	12.832064
13.944309	905.607208	12.837082
14.248372	906.584192	12.842099
14.261046	909.923474	12.847117
14.396724	903.886858	12.852135
14.137542	900.082619	12.857152
14.028358	907.233960	12.862170
14.053745	904.703613	12.867187
14.228387	905.963650	12.872205
14.384474	913.014473	12.877223
14.607540	901.497291	12.882240
13.833300	916.530641	12.887258
14.263848	917.208624	12.892275
14.104084	919.356351	12.897293
14.348035	896.604997	12.902311
14.194223	914.288951	12.907328
14.000408	913.495698	12.912346
14.187668	900.740369	12.917363
13.951081	905.754400	12.922381
14.420541	914.126513	12.927399
14.423901	905.426722	12.932416
14.347713	899.895900	12.937434
14.750560	895.668043	12.942451
14.638793	907.688602	12.947469
14.597813	908.447953	12.952487
14.339522	901.061742	12.957504
14.089197	909.350870	12.962522
14.352054	904.514076	12.967539
14.176383	911.947224	12.972557
14.438796	932.021217	12.977575
14.608550	942.920180	12.982592
14.631129	941.138679	12.987610
14.974211	935.936418	12.992627
14.775241	938.486126	12.997645
14.589635	918.556607	13.002663
14.785227	907.209579	13.007680
14.313137	899.429252	13.012698
14.497795	908.157622	13.017715
14.787553	921.243028	13.022733
14.784678	928.368151	13.027751
15.096976	922.928998	13.032768
14.407444	922.188535	13.037786
14.626779	920.789997	13.042803
14.798315	928.670604	13.047821
14.703625	921.195548	13.052839
14.749820	929.234146	13.057856
14.787369	929.006977	13.062874
15.324820	933.548972	13.067891
14.564084	912.808959	13.072909
14.551152	923.690470	13.077927
14.886614	927.482816	13.082944
14.879323	925.355038	13.087962
15.111917	929.380585	13.092979
15.157224	930.793371	13.097997
14.661210	910.785163	13.103015
15.066003	909.669109	13.108032
14.318624	913.021319	13.113050
15.016041	911.817643	13.118067
15.132523	926.895010	13.123085
14.984941	928.122389	13.128103
15.233624	917.338425	13.133120
15.169695	927.036949	13.138138
14.989063	905.310495	13.143155
15.003164	894.369287	13.148173
14.943058	888.388944	13.153191
14.705520	900.583798	13.158208
14.760902	919.259081	13.163226
14.900047	920.088352	13.168243
15.262379	931.326084	13.173261
15.339537	928.807154	13.178279
15.134397	929.862876	13.183296
14.863636	934.671579	13.188314
14.765311	941.633085	13.193331
15.117933	938.242502	13.198349
15.226993	932.354243	13.203367
15.338078	934.241898	13.208384
15.302612	929.198045	13.213402
15.543874	925.512538	13.218419
15.151643	923.975049	13.223437
15.070394	929.620975	13.228455
15.232010	931.483254	13.233472
15.213190	929.602415	13.238490
15.231096	931.711040	13.243507
15.184482	932.076513	13.248525
14.754211	928.541343	13.253543
15.093059	936.453349	13.258560
15.046140	935.048622	13.263578
14.716754	923.762949	13.268595
14.985100	944.097544	13.273613
15.240836	961.534180	13.278631
15.772521	959.504794	13.283648
15.690580	951.528887	13.288666
15.747449	947.222193	13.293683
15.813600	947.987656	13.298701
15.538788	937.247382	13.303719
15.540250	921.855802	13.308736
15.206015	928.439140	13.313754
15.342332	918.246082	13.318771
15.527797	925.432582	13.323789
15.195234	951.806258	13.328807
15.492566	954.694152	13.333824
15.758522	952.819389	13.338842
15.896380	949.223097	13.343859
15.595590	944.675169	13.348877
15.343191	945.898123	13.353895
15.953134	940.743475	13.358912
15.711806	950.068155	13.363930
15.615066	944.422427	13.368947
15.845092	925.870113	13.373965
15.351945	923.840732	13.378983
15.159139	930.445474	13.384000
15.477140	939.327089	13.389018
15.851667	942.612976	13.394035
16.088844	951.177798	13.399053
15.859472	964.390853	13.404071
16.259594	956.322880	13.409088
15.903500	951.057055	13.414106
15.713446	937.864828	13.419123
15.918360	922.919558	13.424141
15.530859	924.739240	13.429159
15.885977	941.168173	13.434176
15.611725	960.193301	13.439194
15.641218	952.400910	13.444211
15.803772	954.437120	13.449229
15.625807	958.646348	13.454247
15.833655	947.866455	13.459264
15.785102	955.634556	13.464282
15.792900	952.648922	13.469299
15.967618	943.590831	13.474317
15.539430	953.799487	13.479335
16.147624	948.424791	13.484352
15.945461	953.260149	13.489370
16.006569	946.358635	13.494387
15.992632	960.997633	13.499405
16.013250	955.489073	13.504423
16.156860	955.614192	13.509440
16.147610	960.598938	13.514458
15.795451	951.922446	13.519475
15.727299	957.176721	13.524493
15.605486	961.455593	13.529511
16.345347	970.896237	13.534528
16.180951	971.447976	13.539546
16.377889	978.792911	13.544563
16.532240	960.413071	13.549581
16.272046	957.817922	13.554599
16.394274	941.227443	13.559616
16.328110	956.226775	13.564634
16.378179	945.640447	13.569651
16.336956	940.070471	13.574669
16.104941	943.574977	13.579687
16.116968	939.282683	13.584704
16.260478	944.025093	13.589722
16.446386	946.077222	13.594739
16.095241	944.793918	13.599757
16.057597	960.907630	13.604775
16.396301	959.155859	13.609792
16.484471	968.655978	13.614810
16.451793	977.883902	13.619827
16.704946	955.228069	13.624845
16.291364	947.766926	13.629863
16.272370	936.263346	13.634880
16.374005	956.933228	13.639898
16.465235	969.769645	13.644915
16.640589	977.290359	13.649933
16.531880	983.400209	13.654951
16.459432	969.011762	13.659968
16.341469	977.344001	13.664986
16.362571	990.874677	13.670003
16.781306	972.786112	13.675021
16.457588	979.057552	13.680039
16.756689	973.209022	13.685056
16.763205	983.645609	13.690074
16.193047	982.529082	13.695091
16.652235	965.973427	13.700109
16.294888	973.128414	13.705127
16.688279	976.218116	13.710144
16.611060	981.495743	13.715162
16.385580	979.563041	13.720179
16.606097	979.565431	13.725197
16.592417	981.057740	13.730215
16.454270	981.063112	13.735232
16.433724	978.289109	13.740250
16.297270	989.761941	13.745267
16.709538	999.331038	13.750285
16.876025	1007.528408	13.755303
17.177085	1014.977983	13.760320
17.210245	1002.903530	13.765338
16.829093	997.332043	13.770355
17.173811	984.556430	13.775373
16.635861	979.923001	13.780391
16.629648	987.641118	13.785408
17.038247	1002.132684	13.790426
16.923892	993.515966	13.795443
17.211942	1000.904506	13.800461
16.870567	1009.370713	13.805479
17.413425	996.480569	13.810496
16.992692	991.560885	13.815514
16.854208	992.714632	13.820531
16.718233	974.441700	13.825549
16.782784	1001.231344	13.830567
16.893171	1006.090250	13.835584
17.117448	997.527195	13.840602
17.150377	1010.680017	13.845619
17.302054	1006.236991	13.850637
17.161371	1006.577073	13.855655
17.515219	998.464963	13.860672
17.148826	1001.146071	13.865690
17.280780	1015.106795	13.870707
17.226209	1000.739572	13.875725
17.145028	1000.220365	13.880743
17.588256	1002.427974	13.885760
17.216150	984.423835	13.890778
17.116014	982.010068	13.895795
17.377765	993.207784	13.900813
17.490304	1000.228745	13.905831
17.178953	992.224204	13.910848
17.433937	991.033609	13.915866
17.267119	991.106502	13.920883
17.283391	992.183208	13.925901
17.009717	995.979107	13.930919
17.127771	1000.065031	13.935936
17.533285	995.951450	13.940954
17.276177	998.565195	13.945971
17.585061	995.755446	13.950989
17.141639	1004.482467	13.956007
17.373296	1005.149335	13.961024
17.256388	1000.080735	13.966042
17.253877	1000.277139	13.971059
17.558807	998.355582	13.976077
17.580608	1002.536238	13.981095
17.276038	989.041295	13.986112
17.469619	993.183425	13.991130
17.505440	1000.359165	13.996147
17.853980	993.274426	14.001165
17.432659	1009.654708	14.006183
17.336919	998.026879	14.011200
17.696018	1001.732282	14.016218
17.590907	1025.671776	14.021235
18.044650	1032.678287	14.026253
17.838908	1009.765393	14.031271
17.637585	1006.946666	14.036288
17.778363	1001.798481	14.041306
17.835715	1015.577671	14.046323
17.716053	1006.390663	14.051341
17.857387	1007.734546	14.056359
17.640756	1018.860477	14.061376
17.951844	1020.046212	14.066394
17.586291	1029.745147	14.071411
18.083813	1009.646919	14.076429
17.830862	1027.965979	14.081447
18.215962	1017.152612	14.086464
18.182322	1015.719309	14.091482
17.931925	1009.439224	14.096499
17.647316	997.272826	14.101517
18.011275	1009.242107	14.106535
18.093228	1013.493815	14.111552
18.121840	1015.964989	14.116570
17.927479	1011.845241	14.121587
17.980009	1016.667362	14.126605
18.251682	1021.444118	14.131623
17.789255	1016.549029	14.136640
18.205266	1018.856988	14.141658
18.116629	1024.213276	14.146675
18.148348	1020.701130	14.151693
17.991035	1018.173107	14.156711
18.112056	1027.331082	14.161728
18.035092	1007.346787	14.166746
18.030993	1016.646179	14.171763
18.170949	1011.786461	14.176781
17.913597	1015.406863	14.181799
18.126532	1022.116807	14.186816
17.950185	1014.622134	14.191834
17.672414	1015.056413	14.196851
18.232784	1018.371535	14.201869
18.251361	1025.841818	14.206887
18.032696	1022.509509	14.211904
18.320173	1027.579174	14.216922
18.260842	1045.936029	14.221939
18.586801	1031.609713	14.226957
18.447804	1033.538018	14.231975
18.436022	1032.792025	14.236992
18.122138	1017.142772	14.242010
18.491819	1034.156696	14.247027
18.767841	1037.448943	14.252045
18.568671	1046.993447	14.257063
18.469087	1029.071165	14.262080
18.428099	1028.247434	14.267098
18.254253	1042.794846	14.272115
18.450534	1031.684974	14.277133
18.512970	1041.907671	14.282151
18.332296	1047.666412	14.287168
18.961373	1030.758850	14.292186
18.689695	1041.731423	14.297203
18.691329	1038.835851	14.302221
18.610639	1035.977797	14.307239
18.580816	1044.386829	14.312256
18.857901	1039.053339	14.317274
18.673100	1053.615364	14.322291
18.545815	1042.901218	14.327309
18.752937	1040.242900	14.332327
18.470589	1044.739728	14.337344
18.998643	1033.876648	14.342362
18.666564	1040.051972	14.347379
18.851858	1038.574221	14.352397
18.789419	1038.359441	14.357415
18.459219	1042.009699	14.362432
18.880387	1044.478987	14.367450
18.743474	1049.947377	14.372467
18.831522	1042.731678	14.377485
18.728293	1047.234136	14.382503
18.611639	1042.418488	14.387520
19.114161	1040.263619	14.392538
18.874109	1048.603674	14.397555
19.224549	1059.692704	14.402573
19.092266	1049.216347	14.407591
18.919884	1043.048137	14.412608
19.079589	1051.320261	14.417626
19.036631	1055.075291	14.422643
19.410608	1051.551747	14.427661
19.298994	1047.072116	14.432679
19.059355	1044.899759	14.437696
19.364690	1031.844051	14.442714
18.956570	1039.061092	14.447731
19.098497	1041.740079	14.452749
19.019367	1033.646461	14.457767
19.019347	1050.798355	14.462784
19.425079	1064.220168	14.467802
19.533397	1070.303930	14.472819
19.437504	1044.235676	14.477837
19.433698	1034.275208	14.482855
18.971843	1035.843752	14.487872
19.427195	1033.720986	14.492890
19.412374	1036.941238	14.497907
19.076683	1035.514157	14.502925
19.400877	1052.246003	14.507943
19.478315	1069.080939	14.512960
19.438248	1072.600792	14.517978
19.492577	1067.999062	14.522995
19.618224	1070.151407	14.528013
19.402901	1045.487196	14.533031
19.164077	1045.268893	14.538048
19.534213	1068.614651	14.543066
19.192737	1068.297583	14.548083
19.464929	1067.188671	14.553101
19.614261	1068.216134	14.558119
19.387534	1064.339081	14.563136
19.998989	1063.294358	14.568154
19.867448	1067.957184	14.573171
19.767047	1060.201162	14.578189
19.466717	1056.859314	14.583207
19.289086	1068.210882	14.588224
19.928697	1064.370060	14.593242
19.938637	1068.343773	14.598259
19.888638	1068.733820	14.603277
20.006911	1068.982594	14.608295
19.780113	1068.083582	14.613312
19.649736	1059.501555	14.618330
19.677636	1058.587417	14.623347
19.542593	1068.238540	14.628365
19.489005	1057.801623	14.633383
19.541640	1066.610356	14.638400
19.761068	1067.313297	14.643418
19.715551	1060.912733	14.648435
19.675337	1064.017917	14.653453
20.124624	1060.563801	14.658471
19.959313	1052.610476	14.663488
19.977831	1066.868390	14.668506
20.059869	1070.353992	14.673523
19.786453	1063.865520	14.678541
19.796069	1066.735245	14.683559
19.796338	1075.476173	14.688576
20.287343	1083.759893	14.693594
20.272803	1093.569729	14.698611
19.796247	1096.679126	14.703629
20.280270	1085.881937	14.708647
20.396561	1092.961365	14.713664
20.071142	1095.741113	14.718682
20.103440	1090.077156	14.723699
20.125970	1088.369847	14.728717
20.624969	1081.672534	14.733735
20.189897	1095.276523	14.738752
20.669872	1084.873440	14.743770
20.350016	1076.034184	14.748787
20.082952	1054.179307	14.753805
20.518164	1062.165890	14.758823
20.381437	1073.729858	14.763840
20.399247	1055.573714	14.768858
20.030836	1059.389417	14.773875
19.967691	1082.886018	14.778893
20.120221	1075.880377	14.783911
20.712721	1092.077068	14.788928
20.553864	1091.246636	14.793946
20.750101	1087.862280	14.798963
20.791854	1087.645632	14.803981
20.761407	1086.157474	14.808999
20.807326	1088.239547	14.814016
20.736351	1061.729819	14.819034
20.444411	1064.171901	14.824051
20.525367	1058.453663	14.829069
20.391937	1062.150824	14.834087
20.547245	1073.260893	14.839104
20.498563	1069.423498	14.844122
20.716471	1076.577351	14.849139
20.597656	1082.687139	14.854157
20.476268	1075.155800	14.859175
20.560951	1082.926156	14.864192
20.721805	1073.832392	14.869210
20.673345	1088.155323	14.874227
20.281193	1086.800154	14.879245
20.741970	1076.783058	14.884263
20.180893	1086.125233	14.889280
20.559732	1077.789895	14.894298
20.019318	1093.139044	14.899315
20.645536	1111.508453	14.904333
20.743316	1104.856276	14.909351
20.502912	1116.915675	14.914368
20.776854	1115.072343	14.919386
21.006032	1100.686771	14.924403
21.003012	1108.669631	14.929421
21.317336	1112.616083	14.934439
21.115887	1109.982168	14.939456
21.008662	1109.374265	14.944474
21.330322	1116.238694	14.949491
20.968524	1111.944950	14.954509
21.122532	1108.759465	14.959527
21.132052	1121.981889	14.964544
21.064821	1108.295774	14.969562
21.008802	1107.920707	14.974579
20.818301	1115.168738	14.979597
21.105432	1129.063280	14.984615
21.649526	1141.428021	14.989632
21.435837	1125.128742	14.994650
21.435568	1117.142401	14.999667
21.248056	1102.958736	15.004685
21.247264	1110.436984	15.009703
21.422942	1103.441283	15.014720
21.039313	1108.623749	15.019738
21.507805	1121.045054	15.024755
21.253670	1119.144132	15.029773
21.646873	1122.855344	15.034791
21.931037	1130.722462	15.039808
21.279095	1120.184811	15.044826
21.557657	1106.560038	15.049843
21.310616	1124.208172	15.054861
21.667823	1107.193413	15.059879
21.835783	1109.979214	15.064896
21.810284	1110.241710	15.069914
21.885918	1105.572778	15.074931
21.843957	1107.496768	15.079949
21.783549	1112.176094	15.084967
21.645641	1107.350161	15.089984
21.448167	1100.286817	15.095002
21.883000	1098.647568	15.100019
21.589455	1106.387936	15.105037
21.592155	1104.428630	15.110055
21.756105	1113.607904	15.115072
21.396705	1113.332767	15.120090
21.651707	1105.107627	15.125107
21.879930	1102.375547	15.130125
21.940151	1113.086666	15.135143
21.790830	1113.751056	15.140160
21.693224	1109.093628	15.145178
22.078907	1112.718497	15.150195
21.757804	1120.115060	15.155213
21.618651	1117.493484	15.160231
22.046835	1131.030916	15.165248
21.835976	1135.637492	15.170266
21.843091	1126.669775	15.175283
21.482285	1142.237872	15.180301
21.561042	1144.956347	15.185319
21.745509	1138.357930	15.190336
21.943807	1141.100540	15.195354
22.209760	1136.057685	15.200371
21.888469	1131.938313	15.205389
22.149069	1138.195033	15.210407
22.159504	1135.678830	15.215424
22.535964	1138.608496	15.220442
22.447548	1130.869156	15.225459
22.291593	1133.931286	15.230477
22.415008	1132.450763	15.235495
22.209083	1129.262166	15.240512
22.163003	1137.745184	15.245530
22.309431	1136.798365	15.250547
22.290120	1128.004475	15.255565
22.658266	1139.067610	15.260583
22.588870	1136.316412	15.265600
22.402980	1127.965334	15.270618
22.623401	1137.054989	15.275635
22.340985	1132.715252	15.280653
22.251711	1135.206418	15.285671
22.554708	1137.820917	15.290688
22.591665	1134.666186	15.295706
22.798977	1125.667748	15.300723
22.233874	1142.693185	15.305741
22.574758	1140.845479	15.310759
22.597480	1133.425510	15.315776
22.516795	1150.649006	15.320794
22.276398	1143.558884	15.325811
22.399163	1141.150867	15.330829
22.981638	1164.895172	15.335847
23.022804	1164.612293	15.340864
22.830434	1148.219520	15.345882
22.897276	1139.331479	15.350899
22.586544	1141.217618	15.355917
22.708343	1124.644825	15.360935
22.774095	1139.095164	15.365952
22.710303	1161.340234	15.370970
23.082955	1163.663155	15.375987
22.956376	1165.588539	15.381005
23.190289	1165.081320	15.386023
23.212323	1136.698428	15.391040
22.934831	1131.593833	15.396058
23.279467	1129.804357	15.401075
22.756216	1130.297706	15.406093
22.861356	1126.529054	15.411111
23.158082	1123.976563	15.416128
23.084197	1121.647101	15.421146
22.873776	1121.123170	15.426163
22.598482	1141.073044	15.431181
23.006994	1145.830769	15.436199
23.264650	1156.550622	15.441216
23.207564	1161.299088	15.446234
23.295520	1158.372302	15.451251
23.179075	1157.699593	15.456269
23.253040	1160.344072	15.461287
23.323145	1158.631058	15.466304
22.969929	1154.403785	15.471322
23.384597	1153.982620	15.476339
22.929620	1164.566744	15.481357
23.091778	1160.517644	15.486375
23.297647	1151.154924	15.491392
23.373550	1158.197757	15.496410
23.437481	1147.022778	15.501427
23.191591	1157.183433	15.506445
22.928047	1152.952167	15.511463
23.567627	1159.064982	15.516480
23.361480	1181.404460	15.521498
23.762336	1177.354288	15.526515
23.889352	1171.376666	15.531533
23.397696	1155.890092	15.536551
23.651101	1161.888803	15.541568
23.351409	1157.888471	15.546586
23.629637	1162.634863	15.551603
23.990586	1179.504157	15.556621
23.884604	1171.588791	15.561639
24.164682	1154.715642	15.566656
23.661131	1161.396240	15.571674
23.731190	1143.168474	15.576691
23.333519	1151.121708	15.581709
23.220172	1155.003632	15.586727
23.798039	1163.410715	15.591744
24.154174	1179.282152	15.596762
24.226167	1177.578860	15.601779
24.101637	1173.846773	15.606797
23.604132	1158.928785	15.611815
23.844737	1155.300114	15.616832
23.999159	1172.221440	15.621850
24.111830	1170.119760	15.626867
23.847400	1176.795095	15.631885
23.947727	1182.234758	15.636903
24.055653	1175.202591	15.641920
24.086982	1181.531660	15.646938
24.001835	1181.276149	15.651955
23.966400	1184.474646	15.656973
23.929693	1184.816149	15.661991
24.221579	1185.453095	15.667008
23.822150	1186.501283	15.672026
24.479580	1179.925065	15.677043
24.230853	1186.090412	15.682061
24.068463	1175.297835	15.687079
24.260893	1178.963317	15.692096
23.868644	1186.991054	15.697114
23.919670	1191.862192	15.702131
24.301674	1175.873405	15.707149
24.120760	1179.433879	15.712167
24.670295	1209.722775	15.717184
24.569233	1215.401602	15.722202
24.832505	1194.653670	15.727219
24.666094	1193.779802	15.732237
24.337032	1181.017652	15.737255
24.286110	1177.382240	15.742272
24.217579	1195.006073	15.747290
24.382750	1203.295779	15.752307
24.783698	1211.867930	15.757325
24.861012	1205.293292	15.762343
25.054503	1199.698114	15.767360
24.621341	1191.574842	15.772378
25.032739	1179.849192	15.777395
24.927747	1170.750788	15.782413
24.848572	1181.220270	15.787431
25.034637	1179.859289	15.792448
24.858869	1178.173717	15.797466
24.604112	1174.339352	15.802483
24.561053	1173.780478	15.807501
24.383384	1168.596786	15.812519
24.603015	1180.802025	15.817536
24.586709	1205.726467	15.822554
24.555521	1204.402172	15.827571
25.131359	1210.467677	15.832589
24.736457	1212.945397	15.837607
25.228870	1199.025008	15.842624
24.970998	1202.777900	15.847642
24.838362	1203.991611	15.852659
24.839754	1205.927343	15.857677
24.799611	1205.735052	15.862695
24.999442	1214.133584	15.867712
24.901338	1207.358051	15.872730
25.179445	1203.679871	15.877747
24.874096	1212.074105	15.882765
24.940733	1221.037869	15.887783
25.235474	1223.093800	15.892800
25.644518	1229.288041	15.897818
25.380815	1226.885617	15.902835
25.194165	1228.291888	15.907853
25.322738	1223.147516	15.912871
25.794562	1216.186078	15.917888
25.092911	1215.243402	15.922906
25.195264	1217.932601	15.927923
25.493861	1230.730638	15.932941
25.420497	1232.074691	15.937959
25.543900	1218.179641	15.942976
25.617627	1222.461502	15.947994
25.738593	1237.453901	15.953011
25.815524	1219.021006	15.958029
25.299466	1214.664550	15.963047
25.731240	1209.063450	15.968064
25.736699	1223.654519	15.973082
25.418207	1216.879384	15.978099
25.693449	1218.818280	15.983117
25.771315	1221.614069	15.988135
25.897195	1223.738646	15.993152
25.886780	1220.282130	15.998170
25.803462	1221.400699	16.003187
25.682931	1221.175834	16.008205
25.623058	1227.912253	16.013223
26.076950	1231.538082	16.018240
25.703230	1225.519193	16.023258
25.936372	1216.936444	16.028275
26.037737	1220.166270	16.033293
25.637107	1222.070228	16.038311
25.824930	1211.348864	16.043328
25.634557	1223.500062	16.048346
25.850981	1221.430434	16.053363
25.810169	1213.001800	16.058381
25.689176	1216.984790	16.063399
25.783921	1221.633196	16.068416
25.896642	1244.971869	16.073434
25.865693	1246.475423	16.078451
26.259138	1250.792041	16.083469
26.506042	1253.571908	16.088487
26.555058	1259.893560	16.093504
26.379467	1265.910457	16.098522
26.019505	1254.353555	16.103539
26.347422	1255.898183	16.108557
26.375651	1253.210936	16.113575
26.348941	1246.379303	16.118592
26.554364	1255.876954	16.123610
26.589853	1261.007135	16.128627
26.661032	1243.317366	16.133645
26.389382	1257.418127	16.138663
26.748918	1258.577670	16.143680
26.177852	1240.287655	16.148698
26.586395	1250.114078	16.153715
26.602076	1249.855878	16.158733
26.192781	1247.344659	16.163751
26.508437	1248.331363	16.168768
26.742897	1255.932196	16.173786
26.530516	1247.846610	16.178803
26.808844	1244.793677	16.183821
26.530519	1251.785857	16.188839
26.707346	1246.246163	16.193856
26.422812	1249.570667	16.198874
26.298790	1257.185080	16.203891
26.370715	1248.252639	16.208909
26.614596	1257.844903	16.213927
26.920205	1269.908663	16.218944
27.059053	1276.944495	16.223962
27.046271	1276.435920	16.228979
26.956540	1261.754923	16.233997
26.580689	1263.426875	16.239015
26.673222	1266.963043	16.244032
26.386433	1276.893368	16.249050
26.420015	1281.722936	16.254067
26.902638	1275.946310	16.259085
26.706033	1282.546712	16.264103
26.943340	1284.240547	16.269120
27.096504	1307.217964	16.274138
27.246817	1304.378664	16.279155
27.490224	1293.640382	16.284173
27.485761	1305.724116	16.289191
27.990517	1287.626281	16.294208
27.435210	1280.056723	16.299226
27.165847	1270.598083	16.304243
27.754385	1266.524943	16.309261
27.417285	1276.135878	16.314279
27.446717	1266.524337	16.319296
27.535858	1272.169982	16.324314
27.470561	1266.234536	16.329331
27.921892	1269.442754	16.334349
27.849210	1275.333808	16.339367
27.781151	1269.437787	16.344384
27.848252	1269.886526	16.349402
27.826996	1269.301215	16.354419
27.755984	1261.339676	16.359437
27.916856	1260.521544	16.364455
27.479345	1249.727931	16.369472
27.427890	1241.797220	16.374490
27.484547	1263.331896	16.379507
27.960601	1265.758987	16.384525
27.694764	1267.381661	16.389543
27.708456	1269.179957	16.394560
27.872217	1273.552449	16.399578
27.609473	1267.936593	16.404595
27.868760	1272.687921	16.409613
27.585226	1275.769194	16.414631
27.661239	1262.874888	16.419648
27.411447	1264.586431	16.424666
27.522583	1276.296175	16.429683
27.611593	1271.137265	16.434701
27.427797	1292.294855	16.439719
28.056666	1301.587342	16.444736
27.956232	1299.135096	16.449754
27.759891	1298.157523	16.454771
28.181147	1304.196848	16.459789
27.982116	1307.295457	16.464807
28.128841	1309.094605	16.469824
28.281470	1305.936075	16.474842
27.985802	1294.870799	16.479859
28.088705	1298.961276	16.484877
28.241126	1317.166551	16.489895
28.597241	1317.455344	16.494912
28.487288	1320.974010	16.499930
28.677503	1325.133319	16.504947
28.891065	1308.109996	16.509965
28.736527	1301.998959	16.514983
28.526359	1297.891094	16.520000
28.570581	1290.746586	16.525018
28.313857	1299.770525	16.530035
28.256335	1298.319296	16.535053
28.479958	1292.842904	16.540071
28.444787	1281.606264	16.545088
28.822499	1293.824244	16.550106
28.586711	1294.567683	16.555123
28.837707	1282.540169	16.560141
28.606290	1290.694114	16.565159
28.396024	1296.142434	16.570176
28.756850	1316.084840	16.575194
28.686239	1326.332174	16.580211
28.794477	1319.150503	16.585229
28.867450	1313.893260	16.590247
28.719991	1319.382580	16.595264
28.769921	1318.899265	16.600282
28.986264	1323.656130	16.605299
29.197924	1309.516332	16.610317
29.157240	1317.157941	16.615335
28.939674	1322.183724	16.620352
29.275099	1317.783559	16.625370
29.015739	1329.363261	16.630387
29.175402	1317.143168	16.635405
29.419928	1316.674932	16.640423
29.127573	1328.174469	16.645440
29.306088	1317.370921	16.650458
28.923912	1312.670511	16.655475
29.155069	1313.639693	16.660493
29.133561	1319.496327	16.665511
29.060917	1312.092818	16.670528
29.007621	1306.790510	16.675546
28.870334	1315.524291	16.680563
28.833670	1325.527666	16.685581
29.144357	1337.399332	16.690599
29.061581	1343.912850	16.695616
29.473760	1356.852827	16.700634
29.324703	1353.121206	16.705651
29.219691	1343.729835	16.710669
29.429755	1342.533745	16.715687
29.245791	1350.867449	16.720704
29.425988	1342.139467	16.725722
29.585716	1377.821620	16.730739
30.042901	1353.509684	16.735757
30.210678	1355.468719	16.740775
30.288710	1347.490575	16.745792
30.313046	1334.436861	16.750810
30.091689	1339.306018	16.755827
30.088593	1326.034438	16.760845
29.988475	1336.976115	16.765863
30.271889	1336.910640	16.770880
30.206085	1326.160451	16.775898
29.845118	1334.452542	16.780915
30.101636	1333.357224	16.785933
30.205054	1331.567239	16.790951
29.961670	1321.969649	16.795968
30.272186	1327.723788	16.800986
29.827228	1321.347399	16.806003
30.307313	1339.203914	16.811021
30.317749	1339.078449	16.816039
30.163548	1331.498674	16.821056
30.381084	1329.506198	16.826074
30.060834	1318.683907	16.831091
30.150100	1322.867181	16.836109
30.409700	1328.743692	16.841127
29.968285	1345.703644	16.846144
30.328516	1327.162592	16.851162
30.091928	1342.828849	16.856179
30.602005	1338.527749	16.861197
30.476287	1327.657755	16.866215
30.193121	1331.770314	16.871232
30.470441	1326.427338	16.876250
30.515749	1329.917002	16.881267
30.495649	1329.175223	16.886285
30.583670	1336.200980	16.891303
30.574395	1334.844514	16.896320
30.714671	1335.733848	16.901338
30.683942	1342.484200	16.906355
30.143606	1332.631589	16.911373
30.092952	1339.909166	16.916391
29.841076	1358.169296	16.921408
30.472081	1357.698599	16.926426
30.522398	1370.343914	16.931443
30.574278	1367.226426	16.936461
30.590564	1361.267226	16.941479
30.545676	1375.597314	16.946496
31.001326	1380.246157	16.951514
30.821028	1390.518548	16.956531
31.015231	1390.392434	16.961549
31.412598	1391.815380	16.966567
30.925140	1402.943141	16.971584
31.432900	1384.454401	16.976602
31.127595	1399.463275	16.981619
31.292375	1389.698994	16.986637
31.563590	1375.109990	16.991655
31.029562	1375.150275	16.996672
31.328310	1361.103501	17.001690
31.402969	1348.507923	17.006707
31.444025	1354.933276	17.011725
31.067323	1352.615835	17.016743
31.168071	1369.224250	17.021760
31.404605	1378.636730	17.026778
31.563016	1391.917840	17.031795
31.781608	1399.811875	17.036813
31.492199	1385.313538	17.041831
31.353612	1388.358677	17.046848
31.764115	1392.047416	17.051866
31.373865	1396.222169	17.056883
31.262757	1389.846872	17.061901
31.423158	1384.804060	17.066919
31.510279	1398.298500	17.071936
31.700306	1383.611111	17.076954
31.711306	1394.271710	17.081971
31.519512	1400.112624	17.086989
31.582790	1386.263574	17.092007
31.775851	1394.249607	17.097024
32.326164	1393.417891	17.102042
31.447609	1399.576201	17.107059
31.706175	1391.714635	17.112077
31.894128	1386.070313	17.117095
31.669737	1394.416232	17.122112
31.852476	1399.540824	17.127130
31.910857	1410.334331	17.132147
31.957387	1413.250671	17.137165
32.199370	1406.594610	17.142183
32.257983	1406.033097	17.147200
32.189763	1413.294914	17.152218
32.372236	1402.717193	17.157235
32.403142	1398.846389	17.162253
32.543059	1393.744960	17.167271
32.166266	1402.884653	17.172288
32.157935	1401.850812	17.177306
32.195639	1397.727742	17.182323
32.371217	1406.686209	17.187341
32.453066	1401.219036	17.192359
32.165595	1409.138052	17.197376
32.479473	1402.629340	17.202394
32.272850	1409.887653	17.207411
32.152885	1402.578325	17.212429
32.171148	1398.089429	17.217447
31.896985	1423.320968	17.222464
32.710015	1432.203041	17.227482
32.534195	1426.756003	17.232499
32.532422	1423.759952	17.237517
32.650705	1423.209637	17.242535
32.772855	1429.081150	17.247552
32.785227	1424.746150	17.252570
33.011958	1425.732603	17.257587
32.870724	1433.106283	17.262605
33.076760	1424.943584	17.267623
32.699661	1429.920778	17.272640
32.877620	1433.997115	17.277658
32.916917	1421.718889	17.282675
32.801352	1428.952716	17.287693
33.468122	1431.879931	17.292711
32.958295	1436.386417	17.297728
32.845233	1422.443461	17.302746
33.092507	1436.160054	17.307763
33.017416	1424.169784	17.312781
33.093249	1413.305590	17.317799
33.193966	1428.685716	17.322816
33.184396	1442.288483	17.327834
33.592015	1448.598583	17.332851
33.244757	1450.939154	17.337869
33.666820	1440.626691	17.342887
33.515680	1444.031933	17.347904
33.354843	1440.920256	17.352922
33.875317	1441.611552	17.357939
33.530520	1427.623828	17.362957
33.515036	1416.697175	17.367975
33.500462	1418.584399	17.372992
33.425958	1421.652218	17.378010
33.646580	1442.738656	17.383027
33.732921	1446.572302	17.388045
33.616466	1445.744486	17.393063
33.486516	1447.662392	17.398080
33.915135	1437.783822	17.403098
33.544585	1450.696952	17.408115
33.825949	1447.048290	17.413133
33.761112	1445.036135	17.418151
33.845753	1451.127012	17.423168
33.628479	1441.190830	17.428186
34.066666	1444.563635	17.433203
33.720919	1445.251445	17.438221
33.892453	1443.914886	17.443239
34.089553	1450.887833	17.448256
34.152268	1439.487679	17.453274
33.992290	1438.103557	17.458291
34.177329	1440.864552	17.463309
34.217690	1436.064361	17.468327
34.180569	1451.382459	17.473344
34.244754	1473.316716	17.478362
34.622606	1473.063614	17.483379
34.420645	1467.831283	17.488397
34.385972	1451.053517	17.493415
34.146793	1451.023623	17.498432
34.473476	1472.641117	17.503450
34.916385	1476.357783	17.508467
34.712410	1466.044049	17.513485
34.701296	1450.250238	17.518503
34.585021	1443.407141	17.523520
34.638109	1440.055812	17.528538
34.637042	1442.368893	17.533555
34.267796	1445.488770	17.538573
34.614447	1450.886248	17.543591
34.503415	1463.370142	17.548608
34.590319	1471.613486	17.553626
34.654161	1473.975679	17.558643
34.462220	1474.612093	17.563661
34.919984	1470.653411	17.568679
34.979252	1473.726099	17.573696
34.734575	1474.687125	17.578714
35.140085	1471.281291	17.583731
35.026964	1479.593910	17.588749
35.053370	1468.347941	17.593767
35.084157	1473.429962	17.598784
34.773698	1477.100678	17.603802
35.245649	1469.349065	17.608819
34.606610	1474.107589	17.613837
34.898578	1475.765252	17.618855
35.121406	1485.699278	17.623872
35.210183	1499.398425	17.628890
35.199505	1498.573006	17.633907
35.216218	1498.505942	17.638925
35.135750	1501.358454	17.643943
35.410944	1500.365142	17.648960
35.212966	1491.808019	17.653978
35.700074	1491.712623	17.658995
35.304906	1495.671514	17.664013
35.541071	1493.371653	17.669031
35.547487	1501.092369	17.674048
35.754381	1493.706742	17.679066
35.951591	1485.684820	17.684083
35.612368	1491.950664	17.689101
35.851069	1483.098778	17.694119
35.935734	1496.650592	17.699136
35.757838	1498.649252	17.704154
35.955093	1484.659683	17.709171
35.898761	1496.551578	17.714189
35.819658	1488.884130	17.719207
36.215530	1488.442643	17.724224
35.907470	1490.230562	17.729242
36.087274	1490.400287	17.734259
35.804824	1483.685603	17.739277
36.047159	1486.232837	17.744295
36.001359	1482.326664	17.749312
36.097954	1485.456955	17.754330
36.166687	1494.602397	17.759347
35.913657	1502.796044	17.764365
36.179018	1504.263450	17.769383
36.259624	1512.802106	17.774400
36.513471	1517.842164	17.779418
36.424586	1504.423213	17.784435
36.561545	1505.241856	17.789453
36.478945	1505.902321	17.794471
36.460284	1499.150140	17.799488
36.379580	1505.550211	17.804506
36.724436	1502.032166	17.809523
36.448844	1509.962458	17.814541
36.387113	1504.039911	17.819559
36.526308	1493.179755	17.824576
36.787548	1501.690720	17.829594
36.903789	1500.889793	17.834611
36.602057	1505.845108	17.839629
36.593829	1492.536442	17.844647
36.749758	1505.121115	17.849664
36.563564	1503.106371	17.854682
36.799766	1493.417218	17.859699
36.809710	1511.739956	17.864717
36.943650	1529.574576	17.869735
36.764666	1527.638548	17.874752
36.993756	1526.015345	17.879770
37.055211	1525.137262	17.884787
37.015085	1533.685056	17.889805
36.985338	1522.999233	17.894823
37.215491	1530.928625	17.899840
36.868874	1521.123789	17.904858
37.338728	1526.286005	17.909875
37.365696	1531.891633	17.914893
37.210152	1516.288725	17.919911
37.314177	1515.020001	17.924928
37.288850	1529.531618	17.929946
37.567398	1519.634495	17.934963
37.543752	1530.961252	17.939981
37.519633	1523.866900	17.944999
37.621245	1530.560036	17.950016
37.205750	1535.330646	17.955034
37.689842	1528.649089	17.960051
37.431325	1528.725721	17.965069
37.545132	1526.989698	17.970087
37.534588	1540.313422	17.975104
37.095223	1556.689491	17.980122
37.585916	1559.622210	17.985139
37.404239	1565.433762	17.990157
37.726452	1553.646595	17.995175
38.088443	1563.721234	18.000192
38.077637	1563.886638	18.005210
38.221930	1556.626271	18.010227
38.116410	1559.638621	18.015245
38.139289	1563.785300	18.020263
38.523841	1551.000570	18.025280
38.107653	1559.686891	18.030298
38.530259	1553.992315	18.035315
38.356099	1548.253464	18.040333
38.266943	1549.756038	18.045351
38.507015	1553.504866	18.050368
38.149281	1547.621573	18.055386
38.378433	1549.575214	18.060403
38.311279	1537.675459	18.065421
38.468386	1555.972554	18.070439
38.514451	1547.633892	18.075456
38.211037	1548.755199	18.080474
38.259678	1542.256013	18.085491
38.211979	1556.217297	18.090509
38.299672	1566.937182	18.095527
38.865202	1567.161458	18.100544
38.776056	1577.898568	18.105562
38.941872	1575.664249	18.110579
38.913520	1581.841164	18.115597
38.710403	1582.659325	18.120615
39.038480	1570.123839	18.125632
38.706264	1577.087084	18.130650
38.665695	1577.535123	18.135667
39.070116	1574.038317	18.140685
39.271100	1572.583708	18.145703
39.402627	1575.098291	18.150720
39.143447	1587.659122	18.155738
39.363417	1569.876091	18.160755
39.374584	1579.010627	18.165773
39.413141	1575.191263	18.170791
39.458452	1564.806940	18.175808
39.316553	1565.525822	18.180826
39.278935	1563.255055	18.185843
39.143673	1557.585746	18.190861
39.171353	1564.823913	18.195879
39.441251	1564.210947	18.200896
39.284617	1563.812146	18.205914
39.187981	1576.645671	18.210931
39.572709	1573.963817	18.215949
39.207042	1568.933677	18.220967
39.329437	1565.669082	18.225984
39.078624	1573.366800	18.231002
39.613144	1580.871563	18.236019
39.389144	1588.928783	18.241037
39.449706	1596.741569	18.246055
39.893200	1598.635784	18.251072
39.500399	1603.299529	18.256090
39.593864	1592.834405	18.261107
39.935920	1598.193921	18.266125
39.928590	1603.618262	18.271143
39.751505	1593.537169	18.276160
39.582784	1595.664622	18.281178
39.816008	1606.442561	18.286195
40.280125	1623.977289	18.291213
40.159407	1634.066005	18.296231
40.483349	1615.680189	18.301248
40.268755	1623.518186	18.306266
40.522438	1620.045493	18.311283
40.800851	1608.764862	18.316301
40.774411	1599.765412	18.321319
40.548321	1592.646736	18.326336
40.700299	1586.822484	18.331354
40.672762	1585.863841	18.336371
40.643041	1584.705783	18.341389
40.165226	1586.446382	18.346407
40.305562	1576.571669	18.351424
40.438619	1586.178320	18.356442
40.411861	1599.828549	18.361459
40.922891	1602.581956	18.366477
40.605334	1609.974230	18.371495
40.509544	1609.724406	18.376512
40.838804	1608.001582	18.381530
40.859605	1607.641166	18.386547
41.144303	1602.149258	18.391565
40.899181	1612.703732	18.396583
40.986971	1606.852683	18.401600
41.238656	1613.264988	18.406618
40.980395	1614.860268	18.411635
41.402194	1611.356252	18.416653
41.111458	1616.064937	18.421671
41.041008	1611.868750	18.426688
41.173477	1612.321262	18.431706
41.124829	1603.000131	18.436723
41.338771	1613.810391	18.441741
40.986619	1605.841006	18.446759
41.138760	1606.468983	18.451776
41.047117	1624.335087	18.456794
40.982548	1635.947583	18.461811
41.529972	1627.737023	18.466829
41.127134	1641.861586	18.471847
41.642721	1643.774007	18.476864
41.419676	1637.142339	18.481882
41.660952	1644.815655	18.486899
41.738360	1629.816568	18.491917
41.829127	1634.763945	18.496935
41.764841	1640.205977	18.501952
41.600321	1644.895388	18.506970
41.780525	1648.616342	18.511987
42.358181	1656.640321	18.517005
41.831760	1666.952577	18.522023
42.231198	1656.185502	18.527040
42.218192	1670.846377	18.532058
42.346247	1659.807457	18.537075
42.397570	1657.537330	18.542093
42.236934	1655.703751	18.547111
42.391266	1634.514039	18.552128
42.188712	1625.700151	18.557146
42.242381	1637.738916	18.562163
42.358315	1646.021449	18.567181
42.101561	1655.536283	18.572199
42.568214	1663.019826	18.577216
42.224834	1659.616463	18.582234
42.203047	1662.862403	18.587251
42.664198	1652.527003	18.592269
42.526038	1658.740006	18.597287
42.718935	1647.694709	18.602304
42.930619	1664.802365	18.607322
42.863820	1669.584675	18.612339
43.031995	1650.227252	18.617357
42.900029	1650.564036	18.622375
42.849508	1654.127477	18.627392
42.866208	1654.081081	18.632410
42.869185	1663.981878	18.637427
42.873882	1657.722747	18.642445
42.583395	1658.701590	18.647463
42.793913	1658.277542	18.652480
42.977191	1654.630477	18.657498
42.881792	1651.074930	18.662515
42.904472	1659.033163	18.667533
43.013649	1678.032325	18.672551
43.183220	1680.004490	18.677568
43.211798	1690.507095	18.682586
43.150122	1687.687995	18.687603
43.114289	1685.423016	18.692621
43.056889	1696.698789	18.697639
43.242059	1683.168851	18.702656
43.614514	1694.471409	18.707674
43.434343	1691.772270	18.712691
43.758363	1678.539231	18.717709
43.637667	1681.894618	18.722727
43.749691	1687.490185	18.727744
43.879930	1691.164295	18.732762
43.603924	1683.916245	18.737779
43.736242	1694.327900	18.742797
43.608912	1702.631572	18.747815
43.793457	1708.548385	18.752832
43.916713	1711.002358	18.757850
43.850739	1719.159303	18.762867
44.162365	1716.572959	18.767885
44.143476	1713.514925	18.772903
44.011867	1710.917389	18.777920
44.156769	1716.297324	18.782938
44.028135	1703.450836	18.787955
44.238029	1702.857621	18.792973
43.839840	1717.424142	18.797991
44.226216	1716.408704	18.803008
44.531734	1714.147146	18.808026
44.355055	1723.061464	18.813043
44.898827	1732.999497	18.818061
44.511660	1713.798520	18.823079
44.494070	1704.147435	18.828096
44.392164	1720.974538	18.833114
44.440649	1734.010758	18.838131
44.843103	1734.472392	18.843149
44.748962	1741.449510	18.848167
44.648134	1731.445084	18.853184
44.709648	1725.697532	18.858202
44.614871	1737.785312	18.863219
45.215319	1742.391248	18.868237
44.796229	1735.673248	18.873255
44.538509	1730.700206	18.878272
44.956520	1732.469138	18.883290
44.688169	1733.873800	18.888307
45.312612	1737.210775	18.893325
44.952907	1759.330632	18.898343
44.994736	1755.659286	18.903360
45.040638	1754.269062	18.908378
45.061060	1759.588687	18.913395
45.398928	1760.944150	18.918413
45.150002	1754.923717	18.923431
45.465710	1758.277468	18.928448
45.356519	1763.655123	18.933466
45.218348	1761.907965	18.938483
45.402840	1744.305967	18.943501
45.133413	1757.226654	18.948519
45.786424	1772.941394	18.953536
46.150032	1779.475609	18.958554
46.159502	1782.889814	18.963571
46.005281	1765.109149	18.968589
46.020718	1752.304748	18.973607
45.949585	1752.010302	18.978624
46.112383	1748.938573	18.983642
45.771460	1750.094238	18.988659
46.252887	1746.370719	18.993677
46.091772	1750.200064	18.998695
45.888601	1747.259275	19.003712
45.883548	1748.435609	19.008730
46.057656	1757.570879	19.013747
46.257715	1773.000477	19.018765
46.054414	1775.518462	19.023783
45.942770	1781.422840	19.028800
46.347643	1782.372203	19.033818
45.888517	1785.914625	19.038835
46.332424	1768.706684	19.043853
46.091770	1782.048567	19.048871
46.124992	1789.824242	19.053888
46.324202	1798.247013	19.058906
46.306331	1798.908210	19.063923
46.207926	1798.309450	19.068941
46.482702	1796.222428	19.073959
46.720669	1804.134137	19.078976
46.793309	1812.150916	19.083994
46.789968	1824.927898	19.089011
47.268205	1832.582030	19.094029
47.685245	1832.643668	19.099047
47.239146	1815.325104	19.104064
47.528183	1808.060579	19.109082
47.012401	1805.098613	19.114099
47.717201	1780.153822	19.119117
47.232623	1796.737001	19.124135
47.077656	1799.541847	19.129152
47.227949	1790.539258	19.134170
47.055233	1792.645944	19.139187
47.383298	1799.610989	19.144205
47.738692	1799.936719	19.149223
47.371993	1792.136745	19.154240
47.916410	1786.600082	19.159258
47.204634	1796.233891	19.164275
47.664098	1807.771729	19.169293
47.702743	1818.495172	19.174311
47.936993	1824.705551	19.179328
48.051804	1820.979024	19.184346
47.905508	1826.755304	19.189363
47.935225	1816.555255	19.194381
48.074645	1814.299284	19.199399
48.065419	1825.624663	19.204416
47.923366	1808.225748	19.209434
47.990505	1828.085873	19.214451
48.111167	1830.168489	19.219469
48.047349	1833.780423	19.224487
48.030297	1822.355967	19.229504
48.313086	1824.878465	19.234522
47.960565	1831.160815	19.239539
47.957860	1827.025019	19.244557
48.002922	1827.067428	19.249575
48.033700	1828.179585	19.254592
48.382637	1830.156377	19.259610
48.072629	1848.897108	19.264627
48.202959	1847.654322	19.269645
48.517579	1851.548562	19.274663
48.454332	1866.895599	19.279680
48.717031	1861.102942	19.284698
48.822983	1857.084795	19.289715
48.534774	1856.351670	19.294733
48.938355	1843.637955	19.299751
48.550440	1856.177763	19.304768
48.609663	1859.325919	19.309786
48.762959	1881.498365	19.314803
49.287406	1878.475102	19.319821
49.047333	1866.369051	19.324839
48.888593	1868.670067	19.329856
49.498966	1873.572595	19.334874
49.334535	1876.520341	19.339891
49.562126	1864.116563	19.344909
49.393868	1863.132738	19.349927
49.217443	1879.628866	19.354944
49.532226	1861.907971	19.359962
49.684820	1871.431071	19.364979
49.879443	1876.283026	19.369997
49.644933	1871.378141	19.375015
49.517895	1869.023494	19.380032
49.635237	1876.617026	19.385050
49.619441	1866.637432	19.390067
49.676079	1870.991778	19.395085
49.464530	1859.844878	19.400103
49.158559	1862.577654	19.405120
49.623680	1867.945272	19.410138
49.430104	1893.362861	19.415155
49.882865	1891.303298	19.420173
49.900656	1890.401311	19.425191
49.432101	1902.474618	19.430208
49.970438	1888.296642	19.435226
50.012709	1904.689933	19.440243
49.994966	1924.135716	19.445261
50.610748	1923.081765	19.450279
50.709173	1921.857433	19.455296
50.640151	1922.986680	19.460314
50.953365	1929.179329	19.465331
50.582799	1908.566277	19.470349
50.897221	1905.113204	19.475367
50.832045	1903.125844	19.480384
50.909787	1884.596360	19.485402
50.801571	1885.621268	19.490419
51.025711	1887.379742	19.495437
51.134202	1878.559382	19.500455
50.559325	1886.011827	19.505472
50.975381	1877.529966	19.510490
50.897209	1889.173441	19.515507
50.733161	1911.794191	19.520525
51.207834	1912.423797	19.525543
50.900466	1914.717495	19.530560
51.190317	1920.421736	19.535578
51.137757	1922.286956	19.540595
50.974747	1912.712520	19.545613
51.193011	1916.516019	19.550631
51.133933	1923.312053	19.555648
51.064280	1918.060853	19.560666
51.146612	1920.646607	19.565683
51.317081	1940.886803	19.570701
51.579946	1938.358672	19.575719
51.639907	1946.451624	19.580736
51.602017	1941.557920	19.585754
51.758278	1952.225803	19.590771
51.471361	1953.035982	19.595789
52.112646	1950.829720	19.600807
51.531362	1958.096468	19.605824
51.641508	1949.162618	19.610842
51.721396	1953.377335	19.615859
51.683979	1946.013757	19.620877
52.027182	1955.414869	19.625895
52.034161	1978.869758	19.630912
52.249812	1972.600243	19.635930
52.303809	1970.431782	19.640947
51.968601	1979.018153	19.645965
52.338991	1969.554924	19.650983
52.470990	1969.775268	19.656000
51.999956	1978.575599	19.661018
52.009282	1977.902342	19.666035
52.206257	1976.802846	19.671053
52.390308	1965.461180	19.676071
52.311784	1996.775984	19.681088
52.656448	1994.076864	19.686106
53.205242	1994.054337	19.691123
53.196024	1993.407566	19.696141
53.661887	1975.020309	19.701159
53.043133	1966.163599	19.706176
53.093878	1959.193864	19.711194
53.519246	1951.283783	19.716211
53.311103	1952.513966	19.721229
53.216000	1947.064622	19.726247
53.027580	1943.291926	19.731264
53.337162	1956.110012	19.736282
53.059395	1959.319388	19.741299
52.999987	1960.873969	19.746317
53.378827	1951.051915	19.751335
53.695833	1967.294767	19.756352
53.731073	1971.536549	19.761370
53.545931	1953.225995	19.766387
53.245987	1945.220052	19.771405
53.416956	1967.896928	19.776423
53.493225	1972.015408	19.781440
53.376202	1982.075397	19.786458
53.614107	1992.807761	19.791475
53.535341	1984.455637	19.796493
53.794916	1981.335000	19.801511
53.945462	1990.298732	19.806528
54.037510	1984.385820	19.811546
54.304743	1995.979974	19.816563
54.173375	2002.094956	19.821581
54.296841	1989.887398	19.826599
54.544566	2004.404532	19.831616
53.970220	1997.317431	19.836634
54.300721	1998.219460	19.841651
54.164400	2005.779391	19.846669
54.518193	2017.004769	19.851687
54.408152	2009.787202	19.856704
54.346605	2005.489053	19.861722
54.468633	2013.961111	19.866739
54.552155	2035.481407	19.871757
54.592887	2002.213656	19.876775
54.556801	2005.591349	19.881792
54.620192	2021.886600	19.886810
54.830495	2019.576961	19.891827
55.167620	2031.338903	19.896845
55.091194	2031.083904	19.901863
55.038575	2032.557260	19.906880
55.358757	2035.380471	19.911898
55.366792	2044.637046	19.916915
55.222251	2043.756365	19.921933
55.124809	2039.457249	19.926951
55.255542	2036.974557	19.931968
54.995534	2033.049513	19.936986
55.270748	2043.877114	19.942003
55.093494	2035.782944	19.947021
55.716321	2041.467045	19.952039
55.303795	2036.088626	19.957056
55.103422	2035.270315	19.962074
55.292003	2034.614082	19.967091
55.383304	2064.443837	19.972109
55.544669	2059.728366	19.977127
55.806237	2063.799716	19.982144
55.630289	2063.773345	19.987162
55.841325	2066.896457	19.992179
55.565647	2062.310484	19.997197
55.657454	2061.387792	20.002215
55.893891	2083.442078	20.007232
55.980841	2096.099059	20.012250
56.159366	2099.038004	20.017267
56.171675	2099.107477	20.022285
56.462500	2092.027151	20.027303
56.163561	2094.932212	20.032320
56.362859	2083.780242	20.037338
56.700201	2085.330289	20.042355
56.625108	2092.464441	20.047373
56.559993	2087.351001	20.052391
56.575018	2097.341415	20.057408
56.667328	2089.597314	20.062426
56.682569	2075.973472	20.067443
56.817024	2101.985160	20.072461
57.208752	2107.737196	20.077479
57.175130	2113.122561	20.082496
56.886086	2115.227452	20.087514
57.085802	2111.898396	20.092531
56.934262	2116.516323	20.097549
56.926281	2123.244755	20.102567
57.029171	2127.382104	20.107584
57.030876	2124.060179	20.112602
57.415424	2119.319816	20.117619
57.076654	2120.847750	20.122637
57.527334	2115.911046	20.127655
57.291773	2121.034539	20.132672
57.254919	2139.611008	20.137690
57.530898	2129.508627	20.142707
57.527422	2135.950523	20.147725
57.665479	2142.149961	20.152743
57.709158	2138.869516	20.157760
57.758538	2144.973385	20.162778
57.995972	2141.438307	20.167795
57.834665	2144.424953	20.172813
57.935916	2148.016965	20.177831
57.877633	2146.586645	20.182848
58.125948	2158.462563	20.187866
58.427319	2164.277972	20.192883
58.408378	2171.184202	20.197901
58.603371	2175.172893	20.202919
58.412216	2165.326010	20.207936
58.498918	2171.185556	20.212954
58.962174	2170.964785	20.217971
58.374931	2182.439678	20.222989
58.651458	2166.087219	20.228007
58.585730	2173.862906	20.233024
58.624539	2176.845817	20.238042
59.023398	2165.899173	20.243059
58.730001	2166.939347	20.248077
58.461152	2178.314777	20.253095
58.801058	2168.488982	20.258112
58.586683	2173.887113	20.263130
58.864917	2161.009421	20.268147
58.559132	2180.660000	20.273165
58.756127	2189.591176	20.278183
59.016777	2193.147410	20.283200
58.607929	2209.775398	20.288218
58.866544	2197.595535	20.293235
58.966893	2211.804771	20.298253
58.976188	2220.269590	20.303271
59.512399	2219.406509	20.308288
59.774364	2212.679878	20.313306
59.689901	2215.506807	20.318323
59.594041	2228.744250	20.323341
59.649797	2217.533629	20.328359
59.869307	2206.867160	20.333376
59.566358	2215.678033	20.338394
60.164499	2218.438614	20.343411
60.217287	2227.833363	20.348429
60.284718	2225.250679	20.353447
60.559659	2208.593742	20.358464
60.012305	2213.532592	20.363482
60.159141	2196.225841	20.368499
59.867175	2214.872705	20.373517
60.206289	2230.653762	20.378535
60.321402	2232.863322	20.383552
60.537213	2247.739468	20.388570
60.781482	2233.214929	20.393587
60.751881	2233.623383	20.398605
60.828834	2236.710819	20.403623
60.926768	2241.503285	20.408640
60.726125	2238.850145	20.413658
61.001248	2237.229695	20.418675
60.796170	2241.137678	20.423693
60.896809	2238.163320	20.428711
61.109054	2225.268727	20.433728
60.683748	2233.012337	20.438746
60.967805	2226.787512	20.443763
60.842206	2225.112231	20.448781
60.954772	2255.425014	20.453799
61.138582	2263.602184	20.458816
61.265364	2266.155851	20.463834
61.468720	2264.655909	20.468851
61.375191	2268.777727	20.473869
61.148013	2264.220486	20.478887
61.640861	2259.370264	20.483904
61.474394	2263.151214	20.488922
62.012604	2274.105974	20.493939
61.839201	2284.249092	20.498957
61.861852	2294.488349	20.503975
62.232721	2293.105788	20.508992
62.096096	2292.502891	20.514010
62.432491	2276.843310	20.519027
62.549433	2290.319630	20.524045
62.113004	2279.980184	20.529063
62.296042	2266.201883	20.534080
61.946412	2283.690556	20.539098
62.469679	2285.388427	20.544115
62.750914	2281.688614	20.549133
62.521307	2277.939175	20.554151
62.668218	2280.300953	20.559168
62.518223	2288.630729	20.564186
62.323602	2290.409833	20.569203
62.362396	2273.159626	20.574221
62.256902	2290.305235	20.579239
62.544794	2292.947627	20.584256
62.568871	2306.768411	20.589274
63.097953	2318.957668	20.594291
62.801561	2313.678453	20.599309
62.698674	2318.900155	20.604327
62.868326	2322.054762	20.609344
62.710819	2317.841669	20.614362
62.768319	2323.447658	20.619379
63.077614	2337.206771	20.624397
63.418026	2347.044570	20.629415
63.601901	2345.717312	20.634432
63.280201	2343.850822	20.639450
63.737326	2345.443892	20.644467
63.832487	2340.723924	20.649485
63.520264	2341.086376	20.654503
63.857699	2340.921234	20.659520
63.823953	2346.333864	20.664538
63.834640	2342.162059	20.669555
64.076137	2338.065095	20.674573
63.845007	2337.418370	20.679591
63.881731	2350.100394	20.684608
63.939480	2367.134081	20.689626
64.342964	2372.805542	20.694643
64.500788	2366.130500	20.699661
64.541741	2361.241152	20.704679
64.544548	2363.744856	20.709696
64.398203	2370.211639	20.714714
64.597059	2362.456488	20.719731
64.744969	2364.742333	20.724749
64.435163	2366.544022	20.729767
64.726259	2351.896683	20.734784
64.778443	2365.240279	20.739802
64.942602	2354.870231	20.744819
64.945378	2357.102900	20.749837
64.714108	2359.377394	20.754855
65.057629	2357.969034	20.759872
64.857900	2380.721356	20.764890
65.096936	2388.968988	20.769907
65.326656	2384.215747	20.774925
65.535623	2393.840278	20.779943
65.364057	2392.104077	20.784960
65.078229	2394.100609	20.789978
65.315589	2384.152068	20.794995
65.487601	2387.562773	20.800013
65.260307	2380.941129	20.805031
65.480391	2393.340549	20.810048
65.562910	2419.420404	20.815066
65.879792	2414.513984	20.820083
66.018680	2422.177446	20.825101
65.690558	2429.237827	20.830119
66.069187	2411.483315	20.835136
66.041227	2421.846365	20.840154
66.173926	2419.267428	20.845171
66.087374	2415.366571	20.850189
66.149463	2422.156973	20.855207
66.431689	2425.259734	20.860224
66.519197	2438.517051	20.865242
66.366388	2449.670962	20.870259
66.482991	2446.438633	20.875277
66.504286	2427.949516	20.880295
66.528555	2429.995982	20.885312
66.692380	2434.169600	20.890330
66.314822	2446.905991	20.895347
66.584673	2435.264787	20.900365
66.486075	2452.325782	20.905383
66.953119	2459.957475	20.910400
67.055997	2477.840252	20.915418
67.164510	2469.162061	20.920435
67.284358	2458.621327	20.925453
67.314467	2465.217443	20.930471
67.522789	2461.467830	20.935488
67.516878	2465.698637	20.940506
67.450791	2458.223026	20.945523
67.768658	2455.019636	20.950541
67.201909	2455.175942	20.955559
67.487527	2462.074688	20.960576
67.820846	2466.083900	20.965594
67.817437	2493.798026	20.970611
68.044841	2489.369520	20.975629
67.939377	2486.845479	20.980647
68.337367	2484.585853	20.985664
68.282421	2492.768743	20.990682
67.823465	2491.815986	20.995699
67.954972	2477.647423	21.000717
67.826242	2489.798877	21.005735
68.210220	2485.003581	21.010752
68.410108	2484.145872	21.015770
68.363330	2496.859924	21.020787
68.470444	2483.603188	21.025805
68.524364	2488.576021	21.030823
68.584704	2508.226746	21.035840
68.723203	2507.550426	21.040858
68.704722	2499.881313	21.045875
68.981614	2513.623697	21.050893
68.368600	2521.984642	21.055911
68.876956	2510.893884	21.060928
68.737622	2516.302567	21.065946
68.704957	2508.590718	21.070963
69.091842	2517.257850	21.075981
69.409798	2539.445762	21.080999
69.341553	2530.773321	21.086016
69.499615	2536.824545	21.091034
69.334098	2541.547853	21.096051
69.545071	2535.699127	21.101069
69.333762	2534.039550	21.106087
69.532572	2523.012729	21.111104
69.469469	2538.290337	21.116122
69.495378	2547.582840	21.121139
70.051502	2556.636169	21.126157
69.929621	2563.352908	21.131175
69.868641	2556.752127	21.136192
69.524801	2556.034457	21.141210
69.877490	2564.676756	21.146227
70.354747	2569.130482	21.151245
70.519828	2577.946496	21.156263
70.320404	2580.768081	21.161280
70.536193	2587.083781	21.166298
70.618805	2588.143140	21.171315
70.862741	2579.249216	21.176333
71.203248	2590.084325	21.181351
70.853990	2571.889125	21.186368
71.034167	2576.018153	21.191386
71.077556	2572.863640	21.196403
71.246870	2575.586695	21.201421
71.150054	2584.680619	21.206439
71.077906	2586.067104	21.211456
71.002023	2569.824616	21.216474
71.253068	2576.797035	21.221491
71.484946	2574.210738	21.226509
71.256639	2577.565599	21.231527
71.230962	2574.418364	21.236544
71.498032	2571.468012	21.241562
71.263570	2579.362724	21.246579
71.471343	2584.746352	21.251597
71.175248	2590.639002	21.256615
71.678027	2605.717465	21.261632
71.880092	2605.395177	21.266650
71.554960	2606.312680	21.271667
71.658225	2601.761753	21.276685
71.349438	2622.418038	21.281703
71.847652	2621.443313	21.286720
72.401649	2618.259528	21.291738
72.296673	2627.592997	21.296755
72.662802	2618.273376	21.301773
72.622446	2632.263354	21.306791
72.580088	2628.868096	21.311808
73.052921	2611.165303	21.316826
73.121777	2626.848326	21.321843
72.858447	2619.620570	21.326861
72.961867	2620.418441	21.331879
72.361725	2614.995234	21.336896
73.049009	2624.244434	21.341914
72.982425	2619.273569	21.346931
73.050252	2611.154344	21.351949
72.989472	2628.971827	21.356967
73.142942	2633.850507	21.361984
73.372397	2639.246122	21.367002
73.412639	2654.578416	21.372019
73.507322	2654.099475	21.377037
73.400751	2648.780312	21.382055
73.500650	2648.693001	21.387072
73.669479	2633.811091	21.392090
73.527832	2648.779565	21.397107
73.572677	2647.406167	21.402125
73.495604	2646.364705	21.407143
73.660455	2667.656513	21.412160
73.868358	2675.401604	21.417178
73.788128	2689.669465	21.422195
74.297511	2680.557221	21.427213
74.038505	2687.670860	21.432231
73.959132	2671.131028	21.437248
74.205567	2684.298125	21.442266
74.433137	2706.110097	21.447283
74.699907	2706.332985	21.452301
74.363219	2705.132464	21.457319
74.260195	2710.071268	21.462336
74.998977	2693.784180	21.467354
74.655256	2709.459289	21.472371
74.738589	2711.344467	21.477389
74.796406	2726.367451	21.482407
75.147387	2732.350852	21.487424
75.137856	2733.291401	21.492442
75.337584	2741.141806	21.497459
75.579192	2738.815866	21.502477
75.588905	2739.630803	21.507495
75.280230	2734.265682	21.512512
75.370840	2733.738596	21.517530
75.311525	2749.973795	21.522547
75.465277	2743.102820	21.527565
75.715893	2729.999314	21.532583
75.861953	2759.828449	21.537600
76.023652	2763.568480	21.542618
75.626728	2771.162400	21.547635
75.959364	2771.764537	21.552653
76.091835	2763.960907	21.557671
75.775887	2760.681494	21.562688
76.359302	2767.337479	21.567706
76.063896	2768.185121	21.572723
76.290721	2772.786386	21.577741
76.357166	2795.155195	21.582759
76.255042	2800.163560	21.587776
76.518479	2797.306870	21.592794
76.726704	2801.219133	21.597811
76.546440	2797.648803	21.602829
76.675092	2794.196314	21.607847
76.704283	2813.672269	21.612864
77.121565	2813.638017	21.617882
77.000806	2826.781666	21.622899
77.207831	2833.310517	21.627917
77.122924	2822.122112	21.632935
77.058003	2817.819374	21.637952
77.289039	2820.986971	21.642970
77.488433	2830.623986	21.647987
77.573085	2833.862623	21.653005
78.038913	2847.849461	21.658023
77.854543	2841.247296	21.663040
77.896348	2818.959856	21.668058
77.665059	2830.010087	21.673075
77.969903	2832.371048	21.678093
78.002986	2845.791242	21.683111
77.999382	2852.426557	21.688128
78.361210	2834.806810	21.693146
78.053860	2846.886885	21.698163
78.383777	2846.512759	21.703181
78.213885	2843.814276	21.708199
78.096462	2845.682452	21.713216
78.450594	2824.729534	21.718234
78.694652	2848.368206	21.723251
78.532217	2862.764765	21.728269
78.940875	2861.287531	21.733287
78.752396	2871.915386	21.738304
79.277309	2862.426081	21.743322
79.230597	2866.582838	21.748339
79.357664	2875.583838	21.753357
79.401089	2862.328248	21.758375
79.212200	2870.864555	21.763392
79.532228	2870.323175	21.768410
79.558951	2865.304925	21.773427
79.546970	2860.705647	21.778445
79.574496	2859.096129	21.783463
79.208637	2864.592166	21.788480
79.376824	2849.894002	21.793498
79.477905	2879.604037	21.798515
79.650489	2890.306878	21.803533
79.940538	2889.248039	21.808551
79.978663	2900.134121	21.813568
80.100218	2895.952507	21.818586
80.017437	2896.376459	21.823603
79.899237	2904.842445	21.828621
80.188703	2905.785169	21.833639
80.034649	2928.855927	21.838656
80.545369	2928.434207	21.843674
80.009567	2929.171196	21.848691
80.526269	2930.532253	21.853709
80.862267	2940.093223	21.858727
80.411767	2948.927909	21.863744
80.739589	2944.077583	21.868762
80.733611	2942.027947	21.873779
80.650452	2945.096710	21.878797
81.106169	2949.214557	21.883815
80.995881	2966.907152	21.888832
81.152591	2977.576065	21.893850
80.886087	2977.689844	21.898867
80.977598	2977.716905	21.903885
81.535325	2994.927903	21.908903
81.408851	3004.444081	21.913920
81.514408	3002.171291	21.918938
81.695317	3003.772480	21.923955
81.447428	3007.744026	21.928973
81.457651	3014.645222	21.933991
81.871322	3025.684286	21.939008
82.366613	3027.591779	21.944026
82.522615	3027.690463	21.949043
82.643256	3033.830149	21.954061
83.088125	3029.506100	21.959079
82.475655	3031.221073	21.964096
82.955139	3016.245338	21.969114
82.802643	3023.552543	21.974131
82.617765	3023.613860	21.979149
82.853694	3015.710727	21.984167
83.013323	3029.457004	21.989184
83.092345	3014.110457	21.994202
82.967912	3022.448017	21.999219
82.722897	3027.644233	22.004237
83.108161	3016.005963	22.009255
83.047643	3020.979572	22.014272
83.198095	3036.666653	22.019290
83.434538	3045.853212	22.024307
83.356513	3051.829680	22.029325
83.598123	3048.720264	22.034343
83.454895	3063.040215	22.039360
83.207261	3046.043359	22.044378
83.266297	3049.812235	22.049395
83.639073	3085.970003	22.054413
84.039679	3070.231692	22.059431
83.796701	3080.156127	22.064448
83.746238	3084.730868	22.069466
84.141793	3091.640469	22.074483
84.232513	3115.201742	22.079501
84.514878	3106.175581	22.084519
84.591985	3111.758342	22.089536
84.624956	3109.238487	22.094554
84.849006	3111.043574	22.099571
84.328216	3100.659249	22.104589
84.749499	3098.260260	22.109607
84.666680	3116.285481	22.114624
84.827077	3126.317692	22.119642
85.108007	3129.997166	22.124659
85.308713	3141.807697	22.129677
85.599739	3135.934298	22.134695
85.360145	3144.396854	22.139712
85.426074	3133.098263	22.144730
85.462191	3135.541864	22.149747
85.120357	3131.736748	22.154765
85.845206	3136.153861	22.159783
85.827282	3156.829326	22.164800
86.024917	3161.968188	22.169818
86.474435	3164.015148	22.174835
86.273268	3168.650248	22.179853
86.427203	3151.468419	22.184871
86.247776	3157.620732	22.189888
86.402566	3158.125902	22.194906
86.362516	3154.418937	22.199923
86.212555	3146.076375	22.204941
86.172181	3161.045930	22.209959
86.088857	3156.544571	22.214976
86.327994	3182.393540	22.219994
86.551755	3189.744158	22.225011
86.399904	3183.147889	22.230029
86.635141	3184.277539	22.235047
86.956388	3207.592599	22.240064
87.123926	3217.020166	22.245082
87.007080	3217.206063	22.250099
87.236754	3227.881988	22.255117
87.254213	3217.121249	22.260135
87.302096	3223.754514	22.265152
87.403369	3244.408431	22.270170
87.659234	3239.011654	22.275187
87.711575	3244.952088	22.280205
88.397276	3247.922993	22.285223
88.139275	3253.161585	22.290240
88.219092	3246.186074	22.295258
88.281190	3245.318024	22.300275
88.149458	3252.904575	22.305293
88.073271	3249.232298	22.310311
88.358218	3241.569369	22.315328
88.241900	3258.502294	22.320346
88.457259	3264.549651	22.325363
88.522581	3265.338104	22.330381
88.897485	3270.533140	22.335399
88.641718	3281.478290	22.340416
88.859598	3262.968486	22.345434
89.153145	3263.813318	22.350451
88.596948	3269.246856	22.355469
88.851233	3261.142541	22.360487
88.959459	3278.123419	22.365504
88.953136	3299.088880	22.370522
89.596550	3292.117458	22.375539
89.635889	3304.358309	22.380557
89.463183	3295.377710	22.385575
89.462660	3292.399987	22.390592
89.472055	3300.239216	22.395610
89.663522	3313.454121	22.400627
89.817726	3333.835638	22.405645
89.946264	3324.987915	22.410663
90.190814	3325.094804	22.415680
90.036033	3329.633706	22.420698
90.660441	3327.855825	22.425715
90.274077	3337.264368	22.430733
90.575251	3332.458877	22.435751
90.641327	3341.199761	22.440768
90.560866	3356.285181	22.445786
91.218172	3339.602233	22.450803
90.997636	3348.371979	22.455821
90.976803	3353.672593	22.460839
91.227828	3354.342178	22.465856
90.866204	3350.670588	22.470874
91.058809	3348.125496	22.475891
90.984908	3361.568147	22.480909
90.878783	3350.930096	22.485927
91.389380	3362.869898	22.490944
91.107188	3379.707926	22.495962
91.482774	3368.405238	22.500979
91.404919	3377.947861	22.505997
91.715127	3390.564483	22.511015
92.173549	3399.244111	22.516032
92.040132	3403.315341	22.521050
92.487456	3403.126524	22.526067
92.140938	3398.898502	22.531085
92.354200	3401.747903	22.536103
92.295618	3401.071830	22.541120
92.321231	3406.034086	22.546138
92.709096	3408.834165	22.551155
92.682170	3425.759193	22.556173
92.863317	3427.975336	22.561191
92.857521	3422.458353	22.566208
93.152778	3410.832300	22.571226
93.390905	3424.347063	22.576243
93.282485	3440.955266	22.581261
93.245033	3422.460300	22.586279
93.281063	3424.561843	22.591296
93.302931	3428.817258	22.596314
93.540717	3421.950207	22.601331
93.227191	3441.273351	22.606349
93.582546	3452.812900	22.611367
93.570378	3448.973701	22.616384
93.697814	3457.912775	22.621402
93.568798	3457.706992	22.626419
93.497285	3464.976613	22.631437
93.790103	3476.509191	22.636455
94.383685	3481.896900	22.641472
94.027092	3487.183752	22.646490
94.422522	3492.725466	22.651507
94.325531	3519.452969	22.656525
94.689009	3511.510793	22.661543
94.928792	3513.426713	22.666560
94.628576	3524.385284	22.671578
94.690797	3506.424921	22.676595
94.575063	3510.820811	22.681613
94.679752	3529.817087	22.686631
95.445557	3535.736980	22.691648
95.480747	3524.593969	22.696666
95.318193	3537.551033	22.701683
95.284508	3544.139253	22.706701
95.566971	3543.926103	22.711719
95.728804	3522.765836	22.716736
95.412381	3547.109994	22.721754
95.669861	3533.541298	22.726771
96.128012	3556.526785	22.731789
96.283700	3567.491152	22.736807
95.947946	3573.582061	22.741824
96.023503	3574.820802	22.746842
96.232577	3561.850625	22.751859
96.156855	3575.974069	22.756877
95.978272	3578.121332	22.761895
96.737204	3582.977035	22.766912
96.518440	3600.854023	22.771930
96.674744	3594.293666	22.776947
96.898269	3601.864595	22.781965
96.915573	3610.323929	22.786983
96.681822	3599.379634	22.792000
96.828284	3611.081771	22.797018
97.018994	3621.151026	22.802035
96.810323	3630.276841	22.807053
97.133592	3635.244314	22.812071
97.433203	3641.122386	22.817088
97.569524	3664.681290	22.822106
97.638098	3659.590907	22.827123
97.850385	3652.122854	22.832141
97.581725	3659.611363	22.837159
98.094328	3665.989679	22.842176
98.204724	3687.988736	22.847194
98.401684	3690.982617	22.852211
98.134285	3690.975681	22.857229
97.958855	3689.937015	22.862247
98.388060	3684.998842	22.867264
98.310332	3701.364063	22.872282
98.719747	3720.031478	22.877299
99.066537	3713.138019	22.882317
98.966443	3722.708938	22.887335
99.188538	3705.967201	22.892352
98.882946	3718.038999	22.897370
99.178836	3701.003184	22.902387
99.331068	3717.685539	22.907405
99.476631	3736.656811	22.912423
99.614845	3729.431275	22.917440
99.724593	3738.534064	22.922458
99.626306	3745.526351	22.927475
99.810649	3735.731772	22.932493
99.777958	3741.290777	22.937511
100.128783	3747.271844	22.942528
99.949301	3762.420477	22.947546
99.651895	3770.064577	22.952563
100.018025	3771.361619	22.957581
99.820093	3772.825490	22.962599
100.369723	3792.990694	22.967616
100.146287	3807.729703	22.972634
100.637010	3804.038027	22.977651
100.913849	3805.341165	22.982669
100.866051	3820.547229	22.987687
101.480840	3822.078778	22.992704
101.289514	3828.527812	22.997722
101.251278	3830.043647	23.002739
101.795259	3820.486045	23.007757
101.556881	3821.966840	23.012775
101.707457	3816.273877	23.017792
101.729303	3822.638076	23.022810
101.994585	3813.056847	23.027827
101.996012	3810.794060	23.032845
102.013556	3816.656603	23.037863
102.257418	3813.685642	23.042880
102.229139	3806.336795	23.047898
102.149424	3811.033119	23.052915
102.325327	3803.980062	23.057933
102.462056	3816.078058	23.062951
102.571153	3809.897854	23.067968
101.819908	3826.974896	23.072986
102.051243	3835.007251	23.078003
102.044027	3838.978606	23.083021
102.433027	3860.833051	23.088039
102.920240	3883.846899	23.093056
102.978489	3872.228171	23.098074
103.160157	3876.224231	23.103091
103.302654	3886.285483	23.108109
103.278823	3913.676777	23.113127
103.785979	3895.629845	23.118144
103.739720	3905.631748	23.123162
103.717645	3907.867368	23.128179
104.089185	3901.620139	23.133197
103.860727	3903.220563	23.138215
103.869475	3905.660148	23.143232
104.316378	3922.750336	23.148250
104.330250	3925.880818	23.153267
104.518367	3927.766351	23.158285
104.304593	3948.599643	23.163303
104.513503	3931.424798	23.168320
104.793464	3934.707377	23.173338
104.676031	3939.912341	23.178355
105.019918	3947.966708	23.183373
104.748121	3943.916347	23.188391
104.961154	3952.723057	23.193408
105.106507	3958.618867	23.198426
104.787051	3966.791516	23.203443
105.460677	3972.529958	23.208461
105.201582	3987.203769	23.213479
105.597071	3987.591239	23.218496
105.868613	3984.010938	23.223514
105.734309	3995.951100	23.228531
106.047184	3983.987453	23.233549
105.839104	3991.882259	23.238567
106.239858	4010.619567	23.243584
106.334253	4011.242622	23.248602
106.389163	4021.117644	23.253619
106.531408	4003.325377	23.258637
106.640967	4005.542410	23.263655
106.539186	4010.164092	23.268672
106.640908	4023.299549	23.273690
106.833177	4030.065601	23.278707
107.069855	4037.990483	23.283725
106.789984	4043.136888	23.288743
107.067950	4045.620199	23.293760
106.943861	4054.366136	23.298778
106.797352	4076.980647	23.303795
107.296100	4071.848576	23.308813
107.018044	4077.595098	23.313831
107.518289	4096.839311	23.318848
107.942799	4097.617274	23.323866
107.640352	4097.880306	23.328883
108.286454	4099.230329	23.333901
108.004509	4116.610462	23.338919
108.467220	4141.037437	23.343936
108.679752	4137.527483	23.348954
108.382788	4137.936071	23.353971
108.773480	4131.882047	23.358989
108.624519	4140.660489	23.364007
108.792533	4138.230754	23.369024
109.373745	4124.151345	23.374042
109.138248	4137.364668	23.379059
109.196155	4133.127097	23.384077
108.805747	4139.344975	23.389095
108.822321	4152.581621	23.394112
109.086510	4164.934818	23.399130
109.178847	4165.010173	23.404147
109.761726	4170.582971	23.409165
109.497749	4199.025501	23.414183
109.594474	4194.686613	23.419200
109.749117	4196.244236	23.424218
109.848495	4207.508526	23.429235
110.316216	4207.280900	23.434253
110.253487	4225.800951	23.439271
110.283136	4226.407547	23.444288
110.512353	4206.555338	23.449306
110.328153	4223.411943	23.454323
110.748605	4222.212569	23.459341
110.731895	4243.758990	23.464359
111.010686	4249.470257	23.469376
111.103545	4252.105847	23.474394
111.206194	4259.532499	23.479411
111.093068	4250.865134	23.484429
110.936166	4262.736398	23.489447
111.323203	4262.708330	23.494464
111.809370	4263.735572	23.499482
111.471389	4278.100633	23.504499
111.997306	4268.200457	23.509517
112.098292	4286.284459	23.514535
112.578282	4286.941844	23.519552
112.808054	4293.056909	23.524570
112.764030	4287.383725	23.529587
113.171613	4283.833634	23.534605
112.712757	4276.797454	23.539623
112.878552	4284.916859	23.544640
113.225262	4277.390467	23.549658
112.982996	4290.481806	23.554675
113.498506	4272.106276	23.559693
113.401402	4284.473204	23.564711
113.121709	4278.805106	23.569728
113.302897	4281.151686	23.574746
113.268609	4290.403013	23.579763
113.257492	4283.692466	23.584781
113.557204	4294.406375	23.589799
113.515674	4306.812171	23.594816
113.637697	4325.572295	23.599834
113.773082	4320.256476	23.604851
113.927725	4334.425615	23.609869
114.077218	4355.121468	23.614887
114.192818	4350.427042	23.619904
113.763985	4353.579973	23.624922
114.105752	4374.925603	23.629939
114.701290	4367.886420	23.634957
114.418327	4375.305191	23.639975
114.527398	4406.830287	23.644992
115.249446	4406.112189	23.650010
115.175788	4415.342535	23.655027
115.179501	4418.870087	23.660045
115.355135	4422.296788	23.665063
115.129795	4426.330322	23.670080
115.179428	4438.940460	23.675098
115.412037	4457.835233	23.680115
116.084535	4447.158720	23.685133
115.983644	4447.391602	23.690151
115.923845	4468.809622	23.695168
116.177492	4473.062065	23.700186
115.922674	4484.900462	23.705203
116.389373	4472.366116	23.710221
116.660882	4476.999091	23.715239
116.179126	4481.509282	23.720256
116.616963	4493.879719	23.725274
116.842901	4495.760648	23.730291
116.956049	4509.143063	23.735309
117.125824	4491.295689	23.740327
117.117324	4501.200786	23.745344
117.350777	4503.823029	23.750362
117.548375	4515.139820	23.755379
117.712061	4526.302372	23.760397
117.529535	4526.570792	23.765415
117.540186	4530.116122	23.770432
117.803521	4518.256714	23.775450
117.800849	4538.478322	23.780467
117.807379	4543.322434	23.785485
118.255929	4542.018783	23.790503
118.184030	4565.494947	23.795520
118.431568	4555.394515	23.800538
117.986251	4575.368824	23.805555
118.507191	4590.431658	23.810573
118.678383	4581.927375	23.815591
118.828885	4584.188516	23.820608
119.278107	4607.559341	23.825626
119.045778	4616.750273	23.830643
119.455475	4613.052114	23.835661
119.381879	4622.822760	23.840679
119.424844	4622.881077	23.845696
119.949245	4632.388340	23.850714
120.015164	4643.938806	23.855731
120.225614	4645.201410	23.860749
120.363652	4650.393925	23.865767
120.291173	4656.079523	23.870784
120.624394	4642.528453	23.875802
120.385323	4651.081112	23.880819
120.494342	4640.728694	23.885837
120.463641	4644.223005	23.890855
120.478627	4664.177276	23.895872
120.575162	4677.845276	23.900890
120.581308	4671.463226	23.905907
120.958463	4688.675239	23.910925
121.280089	4706.416952	23.915943
121.292850	4712.509377	23.920960
121.242983	4708.346549	23.925978
121.898908	4720.742158	23.930995
121.832863	4724.815592	23.936013
121.977992	4725.329499	23.941031
121.794641	4728.116329	23.946048
121.967591	4730.993113	23.951066
122.082203	4730.836429	23.956083
122.128855	4750.678878	23.961101
122.555070	4750.205333	23.966119
122.104457	4765.583217	23.971136
122.518560	4761.124796	23.976154
122.644683	4770.172330	23.981171
122.781029	4794.047527	23.986189
123.006943	4785.605356	23.991207
122.636035	4797.013142	23.996224
123.012081	4806.180434	24.001242
123.165768	4814.312353	24.006259
123.836736	4817.808484	24.011277
123.664587	4824.841414	24.016295
123.685847	4832.896399	24.021312
124.041204	4846.766678	24.026330
123.842068	4859.426137	24.031347
124.030217	4854.914469	24.036365
124.302801	4849.002531	24.041383
124.268273	4867.549394	24.046400
124.612858	4877.638923	24.051418
124.417707	4891.439959	24.056435
124.826480	4872.726219	24.061453
124.672230	4872.423789	24.066471
125.124284	4889.773266	24.071488
125.239292	4894.922815	24.076506
124.822120	4902.861291	24.081523
124.907938	4895.274557	24.086541
125.394577	4913.676692	24.091559
125.646010	4932.634683	24.096576
125.666996	4946.211457	24.101594
125.794008	4942.268964	24.106611
125.992959	4936.231747	24.111629
126.291755	4935.126447	24.116647
126.401204	4933.541370	24.121664
126.740882	4946.285896	24.126682
126.684694	4957.122856	24.131699
126.766699	4965.845878	24.136717
127.190249	4952.674921	24.141735
127.115652	4958.851962	24.146752
127.210397	4952.900861	24.151770
126.993718	4957.030744	24.156787
127.019122	4959.126376	24.161805
127.110085	4969.755550	24.166823
127.082014	4989.208649	24.171840
127.352780	4984.462408	24.176858
127.834867	5006.740914	24.181875
128.038847	5023.245632	24.186893
127.690107	5007.750858	24.191911
128.128209	5014.819267	24.196928
128.058919	5036.251445	24.201946
128.536950	5045.212247	24.206963
128.264047	5055.544094	24.211981
128.479113	5052.860360	24.216999
128.697072	5062.865412	24.222016
128.841299	5079.914755	24.227034
128.666585	5074.389662	24.232051
129.045677	5079.760225	24.237069
129.478828	5088.911161	24.242087
129.212297	5106.659957	24.247104
129.739173	5102.891137	24.252122
129.819229	5108.984803	24.257139
129.879820	5117.125963	24.262157
130.124765	5119.755863	24.267175
130.064595	5141.251250	24.272192
129.998930	5132.616500	24.277210
129.902275	5145.885691	24.282227
130.038750	5158.086750	24.287245
130.382849	5169.250662	24.292263
130.541139	5179.353452	24.297280
130.966100	5175.069516	24.302298
131.342849	5192.136471	24.307315
130.873195	5185.267817	24.312333
131.383030	5182.912555	24.317351
131.496227	5194.801318	24.322368
131.925628	5177.890274	24.327386
132.042074	5192.834687	24.332403
131.672025	5211.208243	24.337421
132.229219	5208.745536	24.342439
132.373634	5213.386740	24.347456
132.505685	5220.485340	24.352474
132.527555	5222.672544	24.357491
132.766308	5216.499104	24.362509
132.874668	5210.506675	24.367527
132.781884	5214.876415	24.372544
132.806538	5211.409079	24.377562
133.090671	5233.335149	24.382579
133.217502	5239.248680	24.387597
133.376363	5243.226024	24.392615
133.131684	5243.655134	24.397632
133.126683	5243.311497	24.402650
133.251403	5258.327841	24.407667
132.973379	5274.493531	24.412685
133.666435	5266.603109	24.417703
133.721764	5293.888854	24.422720
134.088650	5303.409958	24.427738
134.437610	5292.860753	24.432755
134.153844	5305.276263	24.437773
134.043388	5319.027850	24.442791
134.234723	5329.492637	24.447808
134.450023	5333.167736	24.452826
134.889860	5358.697759	24.457843
134.765331	5364.250467	24.462861
135.074350	5363.317089	24.467879
135.056226	5376.314810	24.472896
135.694147	5392.137915	24.477914
135.928939	5413.833783	24.482931
135.565311	5400.924033	24.487949
135.959686	5388.268611	24.492967
136.144520	5397.257196	24.497984
136.172222	5422.042738	24.503002
136.313966	5426.268654	24.508019
136.092223	5429.277723	24.513037
136.384981	5427.773343	24.518055
136.339935	5444.702374	24.523072
136.740422	5451.193276	24.528090
137.093767	5463.528048	24.533107
137.219500	5459.460821	24.538125
137.011821	5475.147719	24.543143
137.239178	5491.677420	24.548160
137.261427	5492.810544	24.553178
137.301925	5506.029421	24.558195
137.753004	5526.026919	24.563213
137.832033	5514.055466	24.568231
137.938582	5529.641672	24.573248
138.254793	5546.702481	24.578266
138.641311	5539.578406	24.583283
138.112868	5552.338118	24.588301
138.483875	5554.513354	24.593319
138.562575	5568.572133	24.598336
138.898407	5571.705264	24.603354
138.848682	5572.263603	24.608371
138.932788	5590.898426	24.613389
139.316808	5603.359358	24.618407
139.342073	5610.137157	24.623424
139.507654	5618.462829	24.628442
139.712731	5631.414825	24.633459
140.097518	5646.705143	24.638477
140.257081	5643.725325	24.643495
139.899568	5641.640495	24.648512
140.095919	5654.089953	24.653530
140.711224	5662.560262	24.658547
140.777739	5660.136040	24.663565
140.506504	5660.251792	24.668583
140.755895	5667.978924	24.673600
140.954992	5680.736649	24.678618
140.906321	5699.167528	24.683635
141.046402	5697.301295	24.688653
141.234014	5706.877862	24.693671
141.785644	5715.447316	24.698688
141.657392	5724.559485	24.703706
142.092055	5725.086223	24.708723
142.114022	5734.786647	24.713741
142.456509	5745.081443	24.718759
142.600969	5758.125460	24.723776
142.287511	5747.688950	24.728794
142.617686	5762.913199	24.733811
142.408353	5765.937212	24.738829
142.675230	5770.791448	24.743847
143.013731	5780.902256	24.748864
142.691360	5793.383592	24.753882
143.008269	5788.656655	24.758899
143.081408	5795.985359	24.763917
143.515868	5810.229304	24.768935
143.334925	5812.843462	24.773952
143.570573	5824.962504	24.778970
143.908242	5826.442800	24.783987
143.619413	5855.920928	24.789005
143.967982	5852.217620	24.794023
144.490949	5877.101992	24.799040
144.293372	5894.065767	24.804058
144.337470	5887.151287	24.809075
144.292014	5885.389322	24.814093
144.583408	5903.846545	24.819111
144.867645	5914.636972	24.824128
144.960542	5929.053621	24.829146
145.288738	5950.476495	24.834163
145.225835	5941.318327	24.839181
145.607227	5951.560368	24.844199
145.774989	5966.165497	24.849216
146.081674	5969.438189	24.854234
146.019739	5965.994051	24.859251
146.033336	5978.484202	24.864269
146.109058	6003.763194	24.869287
146.512964	5999.524649	24.874304
146.803438	6017.147784	24.879322
146.692851	6027.097490	24.884339
146.716294	6036.477731	24.889357
146.963636	6039.662592	24.894375
147.583771	6062.715581	24.899392
147.198721	6070.415048	24.904410
147.558307	6064.710753	24.909427
147.741417	6077.928205	24.914445
147.660162	6088.116446	24.919463
147.685954	6102.077342	24.924480
147.651768	6122.973628	24.929498
147.752697	6129.052429	24.934515
147.966092	6144.577885	24.939533
148.429319	6166.481970	24.944551
148.751303	6163.496086	24.949568
148.829233	6163.250948	24.954586
149.170630	6185.750871	24.959603
148.965785	6195.366596	24.964621
149.155136	6207.588481	24.969639
149.506488	6208.302259	24.974656
149.736599	6224.036876	24.979674
149.927278	6217.491007	24.984691
150.023165	6226.264020	24.989709
149.993819	6231.848558	24.994727
150.355689	6249.025442	24.999744
150.666628	6271.398215	25.004762
150.926468	6255.975688	25.009779
151.017813	6269.876288	25.014797
150.870365	6269.442368	25.019815
151.285038	6285.452900	25.024832
150.895779	6290.099915	25.029850
151.325395	6294.958926	25.034867
151.381981	6301.521577	25.039885
151.289915	6322.821457	25.044903
151.507340	6325.545102	25.049920
151.581032	6326.775709	25.054938
152.056402	6347.212443	25.059955
152.210748	6356.781517	25.064973
152.411650	6353.262756	25.069991
152.360514	6356.752950	25.075008
152.411585	6388.746815	25.080026
153.078145	6384.261191	25.085043
153.004764	6383.313369	25.090061
152.844410	6377.856319	25.095079
152.827315	6403.177673	25.100096
153.020703	6413.437299	25.105114
153.681261	6413.580222	25.110131
154.028047	6444.527531	25.115149
153.995972	6451.692398	25.120167
154.568795	6440.345464	25.125184
154.557614	6457.184936	25.130202
154.502191	6436.368496	25.135219
154.364071	6439.670683	25.140237
154.615988	6458.443403	25.145255
154.973865	6460.939104	25.150272
154.890172	6471.784803	25.155290
154.998306	6470.146239	25.160307
155.063103	6484.696410	25.165325
155.339331	6497.436543	25.170343
155.804144	6507.393856	25.175360
155.544784	6519.642874	25.180378
156.097312	6520.221047	25.185395
156.341677	6528.576713	25.190413
156.372127	6542.664025	25.195431
156.513766	6537.340518	25.200448
156.344820	6548.087738	25.205466
156.757868	6564.347687	25.210483
156.663856	6571.515755	25.215501
157.025518	6570.039263	25.220519
157.242837	6576.284867	25.225536
157.183505	6604.797567	25.230554
157.553938	6605.514513	25.235571
157.658428	6609.398810	25.240589
157.745951	6614.733421	25.245607
157.990120	6623.868841	25.250624
157.957763	6636.885314	25.255642
158.262976	6628.696427	25.260659
158.571657	6642.704779	25.265677
158.460266	6655.935939	25.270695
158.661628	6647.901235	25.275712
158.509178	6673.069765	25.280730
158.234399	6681.223837	25.285747
158.650484	6684.750309	25.290765
158.683382	6721.302256	25.295783
159.379266	6726.206399	25.300800
159.213750	6748.350646	25.305818
159.311520	6760.184866	25.310835
159.855422	6766.830215	25.315853
160.144909	6781.198624	25.320871
160.536170	6782.126352	25.325888
160.255787	6791.265850	25.330906
160.759747	6805.129460	25.335923
160.776954	6813.429881	25.340941
160.832139	6814.299734	25.345959
161.221532	6840.563485	25.350976
161.258717	6843.650139	25.355994
161.329500	6843.867681	25.361011
161.623961	6854.214853	25.366029
161.538751	6864.801179	25.371047
162.110220	6868.790306	25.376064
161.841098	6887.675621	25.381082
161.890033	6893.866481	25.386099
162.653377	6894.251537	25.391117
162.245849	6908.345390	25.396135
162.715302	6917.686326	25.401152
162.552350	6939.291724	25.406170
163.228512	6940.428345	25.411187
163.476694	6941.420679	25.416205
163.511982	6962.383779	25.421223
163.685188	6962.385934	25.426240
163.529537	6974.843411	25.431258
163.661022	6977.253743	25.436275
163.968848	6971.985324	25.441293
163.979523	6990.022790	25.446311
164.396010	6997.750141	25.451328
164.196648	6991.688959	25.456346
164.650744	7011.379525	25.461363
164.799179	7027.049686	25.466381
164.486139	7035.225225	25.471399
165.407802	7046.799879	25.476416
165.191400	7069.428675	25.481434
165.000385	7069.233475	25.486451
165.258238	7075.367047	25.491469
165.285178	7101.159513	25.496487
165.677667	7112.693278	25.501504
166.156991	7127.681959	25.506522
165.999798	7137.206113	25.511539
166.153776	7139.851388	25.516557
166.299405	7159.138678	25.521575
166.653371	7155.309348	25.526592
166.831924	7183.283678	25.531610
167.282958	7189.909900	25.536627
167.128214	7184.708391	25.541645
166.944844	7194.472390	25.546663
167.486740	7206.430456	25.551680
167.786442	7225.452158	25.556698
168.143830	7251.076070	25.561715
168.371596	7248.857691	25.566733
168.297492	7254.900480	25.571751
168.600145	7256.366620	25.576768
168.853449	7279.296143	25.581786
168.640347	7282.554189	25.586803
169.274148	7283.270969	25.591821
168.992344	7300.127704	25.596839
168.977129	7310.152244	25.601856
169.580042	7324.952937	25.606874
169.665822	7345.067854	25.611891
170.090509	7343.106754	25.616909
170.001568	7350.241259	25.621927
170.095859	7354.907921	25.626944
170.061796	7370.505404	25.631962
170.108556	7379.996004	25.636979
170.474782	7395.588804	25.641997
170.922296	7401.817179	25.647015
171.045800	7403.879995	25.652032
171.020673	7426.687195	25.657050
171.266646	7449.239348	25.662067
171.776974	7452.071523	25.667085
171.492618	7453.315700	25.672103
172.051434	7475.731140	25.677120
172.329152	7483.545455	25.682138
171.785598	7495.737436	25.687156
172.344109	7506.167422	25.692173
172.476690	7521.770599	25.697191
172.850950	7526.316230	25.702208
173.232909	7533.403726	25.707226
172.903422	7537.586786	25.712244
173.280995	7555.468976	25.717261
173.057339	7577.900436	25.722279
173.534161	7575.165940	25.727296
174.018286	7583.553436	25.732314
173.664902	7598.086308	25.737332
174.115095	7609.525056	25.742349
174.002648	7621.309597	25.747367
174.533556	7618.987522	25.752384
174.582606	7634.267520	25.757402
174.680868	7646.008600	25.762420
175.152631	7646.158325	25.767437
175.084515	7654.616628	25.772455
175.183114	7657.387706	25.777472
175.436731	7658.153147	25.782490
175.417472	7685.637300	25.787508
176.070124	7690.711928	25.792525
175.980717	7693.120276	25.797543
176.138409	7687.759864	25.802560
176.046441	7703.785459	25.807578
176.168997	7720.697906	25.812596
176.640135	7731.536281	25.817613
176.304885	7754.814988	25.822631
176.406716	7762.587619	25.827648
176.879045	7773.538453	25.832666
177.050366	7796.049879	25.837684
177.777246	7798.161121	25.842701
178.292415	7814.916648	25.847719
178.189250	7819.814550	25.852736
178.140087	7817.589867	25.857754
178.330774	7843.960584	25.862772
178.508165	7852.329596	25.867789
178.590313	7861.994214	25.872807
178.676977	7857.475619	25.877824
178.888753	7886.849225	25.882842
178.848852	7902.193799	25.887860
179.290446	7905.614734	25.892877
179.210408	7919.842824	25.897895
179.253199	7946.364166	25.902912
179.674846	7952.397769	25.907930
179.838164	7973.632474	25.912948
180.222396	7981.609014	25.917965
180.288195	8000.404873	25.922983
180.560744	8010.166503	25.928000
180.684609	8019.194231	25.933018
180.430258	8041.351814	25.938036
181.075467	8045.444842	25.943053
181.187172	8062.682371	25.948071
180.974399	8080.420113	25.953088
181.401720	8080.895385	25.958106
181.514085	8107.987553	25.963124
182.141617	8128.175415	25.968141
182.292834	8132.952619	25.973159
182.649064	8155.912879	25.978176
182.665303	8157.702098	25.983194
182.836736	8166.167563	25.988212
183.324059	8179.328638	25.993229
183.279202	8187.816463	25.998247
183.449705	8183.485555	26.003264
183.621072	8200.512532	26.008282
183.821336	8218.606712	26.013300
183.818020	8210.601098	26.018317
183.979799	8227.470588	26.023335
183.979811	8248.419957	26.028352
184.803283	8246.923720	26.033370
184.792022	8272.663761	26.038388
184.886453	8275.216676	26.043405
185.183221	8273.991769	26.048423
185.065342	8285.694212	26.053440
185.571392	8304.330263	26.058458
185.622607	8305.961707	26.063476
185.791305	8314.266239	26.068493
185.901735	8343.655862	26.073511
185.838320	8342.110825	26.078528
186.360825	8344.119653	26.083546
186.266574	8371.737106	26.088564
186.526342	8377.733822	26.093581
186.758041	8386.993623	26.098599
187.009009	8411.591811	26.103616
187.040356	8412.839031	26.108634
187.228450	8438.047828	26.113652
187.631053	8442.957658	26.118669
187.554337	8445.283684	26.123687
187.603408	8464.368770	26.128704
188.069606	8475.242342	26.133722
188.180297	8486.201442	26.138740
188.492629	8507.375222	26.143757
188.420897	8515.398229	26.148775
188.304989	8527.143056	26.153792
188.711832	8543.031946	26.158810
188.584580	8561.749311	26.163828
188.983126	8568.662041	26.168845
189.510640	8575.066700	26.173863
189.529997	8612.838227	26.178880
189.530966	8619.249565	26.183898
189.934148	8635.103709	26.188916
189.989886	8656.539051	26.193933
190.760863	8671.576318	26.198951
190.793645	8678.311661	26.203968
191.470544	8690.158759	26.208986
190.851671	8696.818258	26.214004
191.314417	8702.240445	26.219021
191.117543	8719.814016	26.224039
191.419911	8728.639372	26.229056
192.042707	8749.995324	26.234074
191.995553	8773.612295	26.239092
192.403542	8771.656148	26.244109
192.613370	8788.366278	26.249127
192.466134	8806.550840	26.254144
192.564729	8814.933382	26.259162
192.686850	8835.397057	26.264180
192.739234	8846.432990	26.269197
193.302195	8859.487616	26.274215
193.475900	8878.255659	26.279232
193.827587	8888.343450	26.284250
194.184197	8901.188819	26.289268
194.528179	8920.079220	26.294285
194.725717	8927.002478	26.299303
194.741995	8940.868209	26.304320
195.038722	8946.117845	26.309338
194.980482	8960.830040	26.314356
195.172393	8965.744128	26.319373
195.538586	8981.154974	26.324391
195.476223	8992.695957	26.329408
195.746474	9005.020067	26.334426
195.767386	9037.244032	26.339444
196.082446	9037.546484	26.344461
196.509677	9060.725536	26.349479
196.348006	9073.799247	26.354496
196.841757	9073.611390	26.359514
196.727724	9096.715303	26.364532
196.926200	9111.319056	26.369549
197.193651	9134.593931	26.374567
197.313741	9135.951786	26.379584
197.419813	9157.433836	26.384602
197.379493	9179.312673	26.389620
197.823111	9199.538593	26.394637
197.974822	9213.327047	26.399655
198.025696	9237.987934	26.404672
198.910823	9253.326693	26.409690
199.157689	9262.940531	26.414708
199.017104	9276.147980	26.419725
199.505503	9285.358016	26.424743
199.678795	9290.395008	26.429760
199.758362	9296.006740	26.434778
199.855674	9309.690840	26.439796
200.155920	9324.469382	26.444813
200.616292	9318.362888	26.449831
200.693970	9322.686296	26.454848
201.239535	9334.364961	26.459866
201.306467	9352.257975	26.464884
201.137707	9369.361309	26.469901
201.452987	9361.044903	26.474919
201.718071	9380.255297	26.479936
201.886961	9398.030693	26.484954
202.032207	9395.601164	26.489972
201.963771	9401.654860	26.494989
202.476126	9425.025178	26.500007
202.221933	9443.224987	26.505024
202.657348	9450.197390	26.510042
202.870302	9466.503635	26.515060
202.751274	9473.863040	26.520077
203.015568	9495.709310	26.525095
203.343068	9508.472548	26.530112
203.860525	9527.473644	26.535130
203.934524	9531.306985	26.540148
204.145787	9555.286503	26.545165
204.083205	9573.540661	26.550183
204.363752	9578.747494	26.555200
204.733167	9602.557593	26.560218
204.799359	9608.482785	26.565236
204.924191	9631.559033	26.570253
204.997622	9637.691780	26.575271
205.173565	9663.944288	26.580288
205.673960	9676.876807	26.585306
205.859816	9704.394364	26.590324
205.746642	9719.164386	26.595341
206.325622	9731.164718	26.600359
206.092805	9756.237985	26.605376
206.166411	9765.138738	26.610394
206.777326	9780.158611	26.615412
207.166373	9815.738020	26.620429
207.570771	9818.641700	26.625447
207.562619	9837.436984	26.630464
207.899699	9843.202500	26.635482
207.890800	9866.961284	26.640500
208.039049	9877.548853	26.645517
208.622956	9902.210920	26.650535
208.357859	9907.863273	26.655552
208.735694	9925.475550	26.660570
208.871893	9942.669323	26.665588
209.279873	9971.441700	26.670605
209.651012	9976.214633	26.675623
209.362482	9998.850848	26.680640
209.846037	10009.221622	26.685658
210.080012	10024.183486	26.690676
210.439893	10042.185627	26.695693
210.674247	10047.314386	26.700711
210.803809	10073.609104	26.705728
210.864712	10073.183973	26.710746
211.360005	10096.588818	26.715764
211.518814	10108.582450	26.720781
211.961086	10103.287640	26.725799
211.908169	10133.714264	26.730816
212.041226	10137.952335	26.735834
212.373925	10152.604187	26.740852
212.374722	10166.301818	26.745869
212.651476	10161.792914	26.750887
213.061330	10197.797472	26.755904
213.062820	10210.125962	26.760922
213.571885	10219.218120	26.765940
213.532836	10242.203383	26.770957
213.619444	10248.171915	26.775975
213.447116	10261.403540	26.780992
213.759309	10269.135553	26.786010
214.287001	10294.550343	26.791028
214.454587	10317.037600	26.796045
214.765365	10308.715146	26.801063
214.946862	10347.644014	26.806080
215.203016	10340.347530	26.811098
215.310209	10359.031418	26.816116
215.401662	10379.054711	26.821133
215.772872	10389.966564	26.826151
216.090689	10409.618495	26.831168
216.157998	10414.656813	26.836186
216.345450	10432.592569	26.841204
216.379221	10443.425508	26.846221
216.902852	10452.176667	26.851239
216.717210	10485.257718	26.856256
217.040096	10492.601293	26.861274
217.716384	10505.380175	26.866292
217.671198	10538.140363	26.871309
217.659516	10538.975782	26.876327
218.275840	10567.578531	26.881344
218.093622	10578.705629	26.886362
218.722601	10591.809070	26.891380
218.794228	10616.330014	26.896397
218.989416	10634.201698	26.901415
218.981169	10644.361104	26.906432
219.562734	10669.439101	26.911450
219.834001	10683.637608	26.916468
219.891181	10686.943852	26.921485
220.016181	10705.474742	26.926503
220.302906	10731.537397	26.931520
220.639743	10740.583474	26.936538
221.007603	10757.389299	26.941556
221.064393	10780.284662	26.946573
221.096602	10785.344651	26.951591
221.112481	10824.246900	26.956608
221.391903	10836.949825	26.961626
222.070683	10840.393663	26.966644
221.789226	10860.424028	26.971661
222.080462	10884.286770	26.976679
222.027347	10900.800719	26.981696
222.455724	10922.189353	26.986714
222.888930	10951.110577	26.991732
223.282224	10959.083185	26.996749
223.726380	10984.508938	27.001767
223.873950	10993.434392	27.006784
224.056500	11006.836449	27.011802
224.330875	11015.540084	27.016820
224.241909	11039.434365	27.021837
224.846619	11042.244518	27.026855
224.894802	11070.521372	27.031872
224.970691	11088.748863	27.036890
225.293112	11094.268323	27.041908
225.202472	11121.655967	27.046925
225.810937	11134.430807	27.051943
225.738484	11163.639206	27.056960
225.751060	11188.069158	27.061978
226.730158	11184.991900	27.066996
226.781601	11217.270360	27.072013
226.924448	11231.919910	27.077031
227.302369	11251.224202	27.082048
227.422851	11262.400231	27.087066
227.923782	11276.222575	27.092084
227.696790	11292.107861	27.097101
228.002095	11304.409841	27.102119
228.671449	11312.437063	27.107136
228.336865	11325.772787	27.112154
229.069521	11339.274087	27.117172
228.940912	11363.836348	27.122189
229.475521	11368.469253	27.127207
229.795273	11374.852660	27.132224
229.811880	11383.597510	27.137242
229.846943	11391.520020	27.142260
229.824507	11397.632256	27.147277
230.179226	11411.866465	27.152295
230.227395	11438.250923	27.157312
230.636527	11461.210363	27.162330
230.990935	11470.331155	27.167348
231.054019	11488.008977	27.172365
230.982951	11506.014645	27.177383
231.173638	11526.739076	27.182400
231.283802	11554.670943	27.187418
232.137673	11573.254937	27.192436
232.356135	11599.797444	27.197453
232.783419	11608.194896	27.202471
232.298516	11633.089799	27.207488
232.372592	11645.609075	27.212506
232.905142	11667.269038	27.217524
232.818214	11698.288005	27.222541
232.867484	11717.098852	27.227559
233.663341	11745.519637	27.232576
233.599857	11772.791248	27.237594
233.983767	11790.869382	27.242612
234.021999	11823.850023	27.247629
234.638510	11854.979168	27.252647
234.780861	11864.164370	27.257664
235.224620	11892.476575	27.262682
235.754711	11909.415155	27.267700
236.224582	11923.712725	27.272717
236.469304	11946.720507	27.277735
236.537866	11955.782449	27.282752
236.628587	11966.236736	27.287770
236.932206	11988.622717	27.292788
237.230473	11993.732879	27.297805
237.227700	12009.967854	27.302823
237.604322	12021.218688	27.307840
237.732662	12048.443316	27.312858
238.121247	12051.948762	27.317876
238.444714	12074.764095	27.322893
238.585553	12092.310774	27.327911
238.696077	12102.621647	27.332928
239.233267	12115.207367	27.337946
239.211494	12148.894231	27.342964
239.330681	12165.239991	27.347981
239.844417	12177.918659	27.352999
240.081872	12199.331089	27.358016
240.045908	12217.475136	27.363034
240.333035	12233.084963	27.368052
240.646291	12253.655363	27.373069
240.842130	12271.701297	27.378087
241.519214	12292.845835	27.383104
240.939749	12311.523331	27.388122
241.961683	12322.080827	27.393140
242.223809	12339.169703	27.398157
242.123120	12365.804808	27.403175
242.319774	12367.769526	27.408192
242.336584	12396.806272	27.413210
242.631245	12409.470110	27.418228
243.110425	12436.041038	27.423245
243.473064	12443.430153	27.428263
243.817535	12469.406518	27.433280
244.156114	12464.711862	27.438298
244.292553	12493.246073	27.443316
244.500064	12512.774634	27.448333
244.367469	12509.988747	27.453351
245.111263	12527.641906	27.458368
244.795473	12557.320044	27.463386
245.191808	12562.203044	27.468404
245.328865	12572.716248	27.473421
245.839384	12597.165336	27.478439
245.688710	12610.911349	27.483456
245.772437	12619.516574	27.488474
246.190104	12642.380175	27.493492
246.002787	12665.179892	27.498509
246.257274	12688.904059	27.503527
246.790513	12719.330910	27.508544
246.776030	12742.130542	27.513562
247.201680	12762.003895	27.518580
247.396806	12799.665649	27.523597
247.684174	12822.754300	27.528615
248.123783	12842.239398	27.533632
247.924910	12863.544381	27.538650
248.269103	12903.209686	27.543668
248.946979	12915.538010	27.548685
249.002810	12937.190210	27.553703
249.705954	12963.453193	27.558720
249.820566	12986.424078	27.563738
250.353603	12988.592503	27.568756
250.690449	13024.866793	27.573773
250.722426	13035.716744	27.578791
251.312249	13038.398935	27.583808
251.159740	13066.415424	27.588826
251.505599	13066.361492	27.593844
251.747577	13087.814535	27.598861
251.824378	13113.306716	27.603879
252.376173	13135.765953	27.608896
252.341459	13154.089691	27.613914
252.318727	13167.671645	27.618932
252.885247	13192.255776	27.623949
252.848955	13222.870642	27.628967
253.455984	13227.439341	27.633984
253.321443	13258.089415	27.639002
253.971284	13283.384763	27.644020
254.083945	13308.039329	27.649037
254.189490	13338.684555	27.654055
254.142859	13348.874856	27.659072
254.707397	13376.951474	27.664090
255.123872	13391.116566	27.669108
254.971165	13430.926718	27.674125
255.315964	13456.603647	27.679143
255.931485	13465.565827	27.684160
255.759254	13511.641506	27.689178
256.126867	13529.902349	27.694196
256.649332	13547.959565	27.699213
256.464413	13578.287654	27.704231
257.176759	13601.995819	27.709248
257.435082	13624.726409	27.714266
257.567154	13646.962607	27.719284
257.564077	13669.726993	27.724301
258.047481	13701.942993	27.729319
258.301783	13717.354828	27.734336
258.665088	13739.597072	27.739354
259.181201	13761.064021	27.744372
259.411306	13778.328322	27.749389
259.653502	13809.690911	27.754407
259.951357	13817.084272	27.759424
260.217723	13839.292243	27.764442
260.606822	13863.979197	27.769460
260.910329	13884.688805	27.774477
260.918516	13896.296499	27.779495
261.247233	13914.422379	27.784512
261.458239	13923.740022	27.789530
261.889159	13952.934906	27.794548
262.292353	13961.541642	27.799565
262.277896	13969.930586	27.804583
262.770512	13974.318275	27.809600
262.884690	14002.432566	27.814618
263.257701	14008.866530	27.819636
263.758657	14026.332174	27.824653
263.595040	14048.647717	27.829671
263.769185	14045.790399	27.834688
263.879033	14070.405617	27.839706
263.818863	14096.794982	27.844724
264.323953	14111.674099	27.849741
264.384875	14139.515353	27.854759
264.840319	14159.511570	27.859776
264.828308	14187.350773	27.864794
265.216088	14220.440860	27.869812
265.549131	14230.428735	27.874829
265.695027	14245.461871	27.879847
265.755859	14287.336289	27.884864
265.834318	14326.297304	27.889882
266.167785	14341.873149	27.894900
266.734299	14369.256211	27.899917
266.756598	14410.425025	27.904935
267.318276	14435.397932	27.909952
267.538183	14457.431625	27.914970
267.684648	14486.458572	27.919988
268.477169	14521.954939	27.925005
268.460007	14549.612811	27.930023
268.988063	14565.169329	27.935040
269.052576	14593.803432	27.940058
269.323666	14627.083820	27.945076
269.812272	14638.377865	27.950093
269.866896	14670.657176	27.955111
270.386369	14694.914125	27.960128
270.806744	14711.856444	27.965146
270.763999	14748.413201	27.970164
271.049299	14770.868309	27.975181
271.019347	14785.644184	27.980199
271.357842	14821.086994	27.985216
271.793983	14846.086001	27.990234
271.717995	14865.775338	27.995252
272.551118	14875.238162	28.000269
272.629159	14919.470491	28.005287
273.332938	14934.867531	28.010304
273.471667	14958.377760	28.015322
273.228129	14986.623767	28.020340
273.604440	15003.904614	28.025357
273.842170	15030.569335	28.030375
274.661534	15065.047563	28.035392
275.000900	15091.356769	28.040410
274.868700	15099.274058	28.045428
275.623786	15123.188565	28.050445
275.380440	15137.725804	28.055463
275.732852	15150.818781	28.060480
276.271977	15197.233995	28.065498
276.582236	15218.779435	28.070516
276.693644	15227.951960	28.075533
276.977073	15265.555991	28.080551
277.473726	15277.309328	28.085568
277.653372	15306.864923	28.090586
277.714829	15334.225890	28.095604
278.054902	15351.809372	28.100621
278.080426	15381.070646	28.105639
278.600431	15400.889099	28.110656
278.973018	15423.032830	28.115674
279.271297	15445.968968	28.120692
279.335730	15465.787120	28.125709
279.402204	15494.811743	28.130727
279.911633	15509.897879	28.135744
280.211858	15530.528176	28.140762
280.488251	15561.554386	28.145780
281.303953	15573.363968	28.150797
281.160679	15587.350817	28.155815
281.371802	15599.725215	28.160832
282.233408	15621.366062	28.165850
282.215575	15646.846328	28.170868
282.628783	15656.008632	28.175885
282.752955	15679.068421	28.180903
283.019687	15693.755126	28.185920
283.065846	15716.827857	28.190938
283.072910	15737.168012	28.195956
283.919866	15739.653739	28.200973
283.865573	15785.238833	28.205991
284.241367	15798.550684	28.211008
284.411944	15826.846347	28.216026
284.853821	15851.513415	28.221044
284.983479	15870.255907	28.226061
285.135113	15901.700527	28.231079
285.204870	15909.304313	28.236096
285.648120	15934.130455	28.241114
285.318663	15974.023295	28.246132
285.898733	16000.456528	28.251149
286.226190	16039.098386	28.256167
286.236453	16068.645518	28.261184
286.966182	16097.043120	28.266202
287.161276	16139.945009	28.271220
287.348427	16166.771240	28.276237
287.481612	16199.180857	28.281255
287.912818	16236.196910	28.286272
288.498396	16269.631998	28.291290
288.642079	16294.122049	28.296308
289.379399	16324.290263	28.301325
289.244842	16356.843716	28.306343
289.244167	16379.805338	28.311360
289.846702	16415.507434	28.316378
290.006355	16455.093683	28.321396
290.640110	16471.926930	28.326413
290.531280	16510.060413	28.331431
290.999800	16542.941712	28.336448
291.242057	16560.552112	28.341466
291.570272	16608.924253	28.346484
291.946968	16633.513432	28.351501
292.175378	16663.001952	28.356519
292.685426	16684.560446	28.361536
293.345089	16723.968595	28.366554
293.234282	16744.490233	28.371572
293.803690	16772.108539	28.376589
293.657821	16809.178671	28.381607
293.901075	16848.124771	28.386624
294.531783	16866.245022	28.391642
294.698708	16909.036943	28.396660
294.623708	16932.326836	28.401677
295.392622	16960.349079	28.406695
295.685409	16993.093246	28.411712
296.094438	17019.022082	28.416730
296.038929	17047.120785	28.421748
296.825795	17075.906251	28.426765
297.117181	17093.844820	28.431783
297.444908	17109.912855	28.436800
297.961923	17137.072324	28.441818
298.058781	17165.117685	28.446836
298.423514	17184.697591	28.451853
298.653475	17210.093635	28.456871
299.131710	17232.444595	28.461888
299.136368	17257.072532	28.466906
299.414965	17289.602127	28.471924
299.927418	17306.275019	28.476941
300.025051	17317.334476	28.481959
299.788383	17340.708397	28.486976
300.334811	17375.066369	28.491994
300.423085	17393.918311	28.497012
300.557024	17432.392096	28.502029
301.159746	17451.263137	28.507047
301.389697	17476.681661	28.512064
301.581014	17503.772605	28.517082
301.320698	17541.569410	28.522100
302.167500	17577.337705	28.527117
302.866326	17604.589275	28.532135
303.171054	17639.069691	28.537152
303.650865	17656.337819	28.542170
303.629758	17689.494597	28.547188
303.790720	17714.822435	28.552205
304.185137	17734.330315	28.557223
304.168724	17770.757054	28.562240
304.881963	17798.547195	28.567258
304.857719	17824.156411	28.572276
305.492638	17854.170977	28.577293
305.765938	17885.799468	28.582311
305.949783	17916.074659	28.587328
306.469105	17948.247393	28.592346
306.794728	17979.671971	28.597364
307.360037	18001.434277	28.602381
307.803852	18043.710538	28.607399
307.662165	18060.530095	28.612416
308.141456	18091.067310	28.617434
308.371977	18117.555400	28.622452
308.713999	18142.827186	28.627469
309.477852	18165.363931	28.632487
308.969605	18203.888865	28.637504
309.791022	18225.308097	28.642522
309.789072	18267.776793	28.647540
309.882572	18284.469453	28.652557
310.342789	18318.517357	28.657575
310.632673	18345.479909	28.662592
310.981634	18374.782920	28.667610
311.393868	18415.884747	28.672628
311.791856	18438.316804	28.677645
312.156744	18467.453419	28.682663
312.185962	18502.792923	28.687680
312.787369	18523.405596	28.692698
312.976626	18555.396029	28.697716
313.113218	18596.576945	28.702733
313.433484	18624.958298	28.707751
313.804570	18660.203829	28.712768
313.989564	18693.385315	28.717786
314.134211	18729.871098	28.722804
314.487822	18763.642767	28.727821
314.926655	18795.447414	28.732839
315.693578	18825.517601	28.737856
315.871684	18860.831695	28.742874
316.313742	18887.437394	28.747892
316.252320	18911.708284	28.752909
316.721541	18937.575024	28.757927
316.824781	18980.571989	28.762944
317.188215	19000.428542	28.767962
317.547536	19031.788076	28.772980
317.869880	19081.156776	28.777997
318.677911	19105.673657	28.783015
318.814097	19135.497093	28.788032
319.000370	19164.353909	28.793050
319.300109	19188.710558	28.798068
319.681196	19231.189374	28.803085
319.966881	19250.642923	28.808103
320.379647	19283.786384	28.813120
320.630218	19323.055529	28.818138
320.652053	19338.753815	28.823156
321.097955	19375.530159	28.828173
321.081007	19401.107503	28.833191
321.498200	19441.766529	28.838208
321.683939	19464.088442	28.843226
322.316720	19506.870025	28.848244
322.409611	19537.598278	28.853261
323.039624	19562.692240	28.858279
323.367770	19598.973066	28.863296
323.705760	19630.565828	28.868314
324.056006	19655.570583	28.873332
324.394399	19691.824697	28.878349
325.075697	19709.359620	28.883367
325.015564	19740.939546	28.888384
325.247078	19776.185284	28.893402
325.619891	19799.433600	28.898420
325.917149	19833.798440	28.903437
326.216200	19866.246174	28.908455
326.548624	19898.611215	28.913472
326.882565	19929.959298	28.918490
327.019903	19968.592896	28.923508
327.335417	20002.140073	28.928525
327.650667	20048.230764	28.933543
328.013050	20081.379410	28.938560
328.594233	20116.588595	28.943578
328.749695	20150.769429	28.948596
328.901405	20174.819356	28.953613
329.001084	20224.185671	28.958631
329.380724	20268.097184	28.963648
329.984195	20288.237212	28.968666
330.506468	20336.509371	28.973684
330.661525	20370.507857	28.978701
331.173981	20405.700631	28.983719
331.477759	20443.144424	28.988736
331.922136	20477.166269	28.993754
332.221832	20500.506467	28.998772
332.599004	20539.861611	29.003789
333.260358	20576.324409	29.008807
333.605660	20615.562033	29.013824
334.124426	20629.066993	29.018842
334.153666	20665.661214	29.023860
334.220079	20706.324526	29.028877
334.660156	20717.477865	29.033895
335.113167	20762.556176	29.038912
335.262258	20791.863365	29.043930
335.682637	20827.433252	29.048948
335.703711	20843.490940	29.053965
336.209320	20887.804191	29.058983
336.050425	20930.023417	29.064000
336.602557	20964.400504	29.069018
337.349496	21014.524561	29.074036
337.538770	21034.716579	29.079053
338.146568	21076.945093	29.084071
338.320780	21115.644618	29.089088
338.576472	21158.705569	29.094106
338.886852	21190.641642	29.099124
338.723813	21223.319699	29.104141
339.313568	21261.258823	29.109159
340.023533	21320.612512	29.114176
340.474603	21336.542880	29.119194
340.955536	21361.069836	29.124212
340.958322	21407.873308	29.129229
341.486818	21425.045885	29.134247
341.998228	21474.338411	29.139264
342.231814	21484.597800	29.144282
342.548761	21516.341073	29.149300
342.922972	21555.109471	29.154317
343.668590	21589.704972	29.159335
343.969780	21613.054360	29.164352
344.379739	21634.730434	29.169370
344.289266	21646.925857	29.174388
344.675551	21685.938505	29.179405
345.071026	21696.330511	29.184423
345.075244	21725.786238	29.189440
345.589022	21764.000763	29.194458
345.865603	21790.290018	29.199476
346.140580	21826.997529	29.204493
346.873199	21852.234071	29.209511
346.875159	21882.715217	29.214528
347.365215	21914.700240	29.219546
347.447633	21947.581947	29.224564
347.447018	21986.597724	29.229581
348.332345	22008.788546	29.234599
348.322948	22057.117242	29.239616
348.421764	22095.352200	29.244634
349.038790	22130.534482	29.249652
349.107950	22178.232523	29.254669
349.742980	22217.936856	29.259687
349.668724	22256.046263	29.264704
350.007942	22286.505533	29.269722
350.979860	22337.140312	29.274740
351.054233	22383.332406	29.279757
351.564057	22412.708962	29.284775
351.932624	22453.350239	29.289792
352.229674	22490.665706	29.294810
352.652657	22519.963774	29.299828
353.284565	22554.991555	29.304845
353.782119	22592.743962	29.309863
354.113042	22618.368077	29.314880
354.271136	22655.793581	29.319898
355.103244	22692.526037	29.324916
354.995756	22727.617990	29.329933
355.632908	22754.555527	29.334951
355.712725	22788.030550	29.339968
356.089066	22825.216986	29.344986
356.655249	22864.776555	29.350004
356.879159	22898.997405	29.355021
357.451274	22920.785523	29.360039
357.655664	22967.804410	29.365056
357.978045	23004.944974	29.370074
358.478398	23040.077485	29.375092
358.502479	23073.155497	29.380109
359.058234	23102.484676	29.385127
359.222613	23139.183362	29.390144
359.177132	23170.442520	29.395162
359.913611	23207.177707	29.400180
360.212137	23241.481527	29.405197
360.625196	23301.827823	29.410215
361.155394	23332.180175	29.415232
361.252638	23347.245380	29.420250
361.706825	23396.575067	29.425268
362.085369	23445.625701	29.430285
362.506193	23464.814282	29.435303
363.012016	23513.091990	29.440320
363.023833	23543.822053	29.445338
363.596497	23576.316908	29.450356
363.816648	23622.321175	29.455373
364.460741	23656.852563	29.460391
364.732212	23694.450846	29.465408
364.989644	23737.021431	29.470426
365.541054	23769.452369	29.475444
365.665914	23814.427516	29.480461
366.150273	23836.117789	29.485479
366.544310	23873.697799	29.490496
366.682764	23921.086576	29.495514
367.324484	23948.365848	29.500532
367.297703	23993.954656	29.505549
367.899037	24023.303134	29.510567
367.932931	24065.007981	29.515584
368.336009	24105.194998	29.520602
368.978712	24139.144193	29.525620
369.009822	24186.346462	29.530637
369.374978	24228.225621	29.535655
369.912867	24254.959626	29.540672
370.292229	24291.458153	29.545690
370.709152	24330.172265	29.550708
371.166290	24368.521888	29.555725
371.813937	24395.316823	29.560743
372.193356	24437.489005	29.565760
372.330897	24469.650641	29.570778
372.799591	24497.050837	29.575796
373.120540	24537.208294	29.580813
373.102641	24575.253693	29.585831
373.714995	24619.100274	29.590848
373.903840	24665.897803	29.595866
374.533831	24705.238264	29.600884
374.532134	24753.251713	29.605901
375.122146	24784.615428	29.610919
375.420754	24833.222844	29.615936
375.798940	24868.647398	29.620954
376.290375	24900.439169	29.625972
376.577785	24957.067087	29.630989
376.916106	25001.920234	29.636007
377.390900	25036.876618	29.641024
377.409113	25081.412292	29.646042
377.818464	25122.199889	29.651060
378.170686	25176.357907	29.656077
378.563208	25217.399237	29.661095
379.296193	25267.877278	29.666112
379.346136	25325.382976	29.671130
380.045097	25355.504501	29.676148
380.381367	25413.384226	29.681165
380.630732	25457.672968	29.686183
381.232253	25492.729198	29.691200
381.415133	25547.621248	29.696218
381.861785	25590.240907	29.701236
382.364742	25637.843903	29.706253
382.888964	25681.198436	29.711271
383.422399	25710.275625	29.716288
383.603695	25755.587195	29.721306
384.471769	25790.480158	29.726324
385.054273	25827.683274	29.731341
385.425980	25867.685674	29.736359
385.624377	25902.591725	29.741376
386.012316	25943.414786	29.746394
386.284183	25984.307582	29.751412
386.566186	26010.804347	29.756429
386.962312	26055.685408	29.761447
387.610474	26092.987066	29.766464
387.817869	26132.802763	29.771482
388.524261	26158.274008	29.776500
388.504936	26207.589149	29.781517
388.842683	26238.328579	29.786535
389.163374	26265.506909	29.791552
389.703778	26316.180718	29.796570
390.261373	26350.880109	29.801588
390.506315	26387.192439	29.806605
390.873035	26429.657082	29.811623
391.339196	26462.416331	29.816640
391.366247	26498.522035	29.821658
392.077462	26534.609413	29.826676
392.447356	26588.094029	29.831693
392.567614	26634.167087	29.836711
392.964728	26661.752907	29.841728
393.485098	26708.759896	29.846746
393.676211	26742.892969	29.851764
393.969932	26780.582701	29.856781
394.170406	26824.346868	29.861799
394.983304	26860.298282	29.866816
395.253413	26910.592701	29.871834
395.553971	26952.952869	29.876852
395.971694	26991.997761	29.881869
396.183597	27030.915883	29.886887
396.638492	27067.504072	29.891904
396.922943	27117.809345	29.896922
397.318160	27169.544211	29.901940
397.660313	27215.055432	29.906957
397.985850	27262.726950	29.911975
398.418633	27315.086876	29.916992
398.749584	27355.837553	29.922010
399.266071	27396.131866	29.927028
399.860029	27451.865773	29.932045
400.131010	27498.294749	29.937063
400.639306	27546.851577	29.942080
400.932080	27604.058272	29.947098
401.600719	27643.665647	29.952116
401.822961	27690.106346	29.957133
402.249442	27737.005490	29.962151
402.723119	27775.052490	29.967168
402.892628	27829.949318	29.972186
403.388604	27889.195730	29.977204
403.995675	27920.291117	29.982221
403.992709	27983.660885	29.987239
404.625013	28011.531757	29.992256
405.090174	28083.110847	29.997274
405.456157	28128.185252	30.002292
405.845041	28175.643802	30.007309
406.402924	28210.315361	30.012327
407.080952	28265.142186	30.017344
407.048930	28309.241885	30.022362
407.624189	28359.149457	30.027380
407.959454	28408.579505	30.032397
408.081993	28467.201942	30.037415
408.530710	28513.844021	30.042432
409.064667	28575.669943	30.047450
409.415545	28629.580419	30.052468
409.986610	28677.704219	30.057485
410.415888	28722.958984	30.062503
411.260610	28767.243075	30.067520
411.127981	28822.640894	30.072538
411.861508	28855.269055	30.077556
412.597457	28899.416887	30.082573
412.609335	28953.885929	30.087591
413.341367	28985.432607	30.092608
413.663293	29052.055331	30.097626
414.139871	29092.953239	30.102644
414.357121	29135.638512	30.107661
414.418391	29186.721675	30.112679
415.059273	29235.065770	30.117696
415.441234	29278.187896	30.122714
416.022977	29327.589314	30.127732
416.232391	29378.475071	30.132749
416.446134	29427.278268	30.137767
416.951660	29478.036537	30.142784
416.892262	29541.556968	30.147802
417.319747	29589.397873	30.152820
418.086523	29639.309043	30.157837
418.053276	29705.724807	30.162855
418.951061	29761.267705	30.167872
419.522919	29816.236856	30.172890
419.608022	29864.302269	30.177908
420.107279	29925.214433	30.182925
420.653044	29970.011560	30.187943
421.400747	30024.069022	30.192960
421.949430	30078.358271	30.197978
422.272361	30117.432193	30.202996
422.622202	30151.861242	30.208013
422.704698	30190.293636	30.213031
423.301969	30246.102245	30.218048
423.810129	30290.187141	30.223066
424.050396	30339.102082	30.228084
424.740102	30391.700176	30.233101
424.932964	30438.591594	30.238119
425.287453	30478.137474	30.243136
426.072786	30539.954103	30.248154
426.458174	30591.353795	30.253172
426.846574	30631.156264	30.258189
426.911173	30689.514991	30.263207
427.544292	30734.675073	30.268224
427.868357	30788.514649	30.273242
428.206129	30845.405965	30.278260
428.612812	30898.118590	30.283277
428.991397	30953.921421	30.288295
429.328166	31010.258192	30.293312
429.746114	31057.416952	30.298330
430.181602	31111.251735	30.303348
430.826995	31166.610506	30.308365
431.006814	31238.871234	30.313383
432.000527	31300.889595	30.318400
432.206548	31354.236168	30.323418
432.537139	31398.523559	30.328436
433.115115	31455.490755	30.333453
433.594826	31506.120378	30.338471
434.222310	31545.153495	30.343488
434.798345	31602.512700	30.348506
435.162044	31659.471787	30.353524
435.720924	31694.071261	30.358541
436.244982	31759.052448	30.363559
436.588989	31806.206508	30.368576
436.685538	31851.975525	30.373594
437.395960	31899.810728	30.378612
437.696191	31954.784155	30.383629
437.802106	32017.058976	30.388647
438.239869	32066.523485	30.393664
438.939662	32122.160240	30.398682
439.356246	32173.824445	30.403700
439.926557	32229.015983	30.408717
440.214544	32291.198599	30.413735
440.972200	32334.316692	30.418752
441.313268	32399.210583	30.423770
441.432432	32451.167673	30.428788
442.225676	32507.998609	30.433805
442.359664	32569.469354	30.438823
443.099719	32615.130901	30.443840
443.431292	32675.553433	30.448858
443.556631	32734.943805	30.453876
444.231179	32781.225544	30.458893
444.322413	32828.821649	30.463911
444.797826	32888.416587	30.468928
445.243570	32955.396569	30.473946
445.427927	33019.375232	30.478964
445.983697	33063.538121	30.483981
446.304728	33130.510972	30.488999
446.652416	33209.535749	30.494016
447.079816	33273.462564	30.499034
448.071427	33335.945968	30.504052
448.683263	33396.378310	30.509069
448.987702	33452.046711	30.514087
449.531469	33494.912696	30.519104
450.104160	33558.706108	30.524122
450.323012	33609.280747	30.529140
451.137941	33657.466323	30.534157
451.150006	33715.667067	30.539175
451.609271	33777.858179	30.544192
451.909174	33818.026414	30.549210
452.230111	33876.369140	30.554228
452.791683	33932.564537	30.559245
452.945608	33994.223108	30.564263
453.863804	34051.764108	30.569280
454.243181	34108.703272	30.574298
454.553163	34162.227334	30.579316
455.243761	34214.003705	30.584333
455.018769	34270.364811	30.589351
455.185674	34345.776872	30.594368
456.256782	34411.321166	30.599386
456.759329	34478.786621	30.604404
457.249388	34542.313234	30.609421
457.210282	34612.494006	30.614439
457.958930	34670.986418	30.619456
458.536741	34744.341189	30.624474
458.512109	34808.259853	30.629492
459.184693	34871.208434	30.634509
459.952981	34933.374636	30.639527
460.394152	35014.070747	30.644544
461.066006	35070.942593	30.649562
461.425096	35138.342735	30.654580
462.497654	35202.393975	30.659597
462.877103	35260.217219	30.664615
463.359107	35320.948943	30.669632
463.367380	35381.702326	30.674650
463.567667	35440.609720	30.679668
464.565048	35501.708180	30.684685
464.815331	35562.734608	30.689703
465.077684	35629.458346	30.694720
465.600128	35692.406228	30.699738
466.203377	35765.956652	30.704756
466.668305	35822.038289	30.709773
467.079478	35887.775926	30.714791
467.549149	35952.185058	30.719808
468.210247	36015.167977	30.724826
468.695519	36078.170693	30.729844
469.403501	36140.000779	30.734861
469.950997	36198.913278	30.739879
470.249940	36264.898052	30.744896
470.737305	36314.505071	30.749914
471.230234	36384.945744	30.754932
471.928591	36429.077667	30.759949
472.071903	36496.458613	30.764967
472.482666	36566.998780	30.769984
473.037782	36620.458167	30.775002
473.328304	36691.056554	30.780020
473.596930	36761.251730	30.785037
474.112595	36827.641438	30.790055
474.268238	36889.934583	30.795072
475.214604	36951.519806	30.800090
475.562751	37036.352512	30.805108
475.872926	37096.051949	30.810125
476.515355	37163.072073	30.815143
476.634293	37239.088101	30.820160
477.399482	37308.802589	30.825178
477.600938	37385.159068	30.830196
477.966632	37451.411742	30.835213
478.908374	37525.633029	30.840231
479.209732	37595.024433	30.845248
479.623704	37662.970988	30.850266
480.121331	37744.089814	30.855284
480.865099	37803.751535	30.860301
481.252789	37860.196305	30.865319
481.861894	37935.525187	30.870336
482.521864	37990.558819	30.875354
482.757847	38046.757811	30.880372
483.434606	38114.258682	30.885389
483.786440	38174.986848	30.890407
484.307565	38221.964528	30.895424
485.064537	38278.920863	30.900442
485.444838	38341.459651	30.905460
485.675932	38391.960569	30.910477
486.394749	38458.123892	30.915495
486.605406	38533.353806	30.920512
487.422992	38582.284456	30.925530
487.786890	38650.015751	30.930548
488.060623	38718.914201	30.935565
488.965076	38781.604644	30.940583
489.407161	38843.939278	30.945600
489.839411	38909.343596	30.950618
490.004092	38965.169000	30.955636
490.774979	39026.351582	30.960653
491.251720	39086.721301	30.965671
491.195272	39164.949050	30.970688
492.271488	39232.249234	30.975706
492.357896	39298.248646	30.980724
493.122406	39362.075226	30.985741
493.687101	39436.480268	30.990759
493.942294	39508.698905	30.995776
494.721676	39569.354808	31.000794
495.293925	39619.850138	31.005812
495.949953	39691.659251	31.010829
496.403799	39746.441883	31.015847
496.855687	39808.989685	31.020864
497.478706	39870.691932	31.025882
497.839615	39944.750792	31.030900
497.979773	40013.758280	31.035917
498.829983	40074.760845	31.040935
498.797572	40141.038607	31.045952
499.749443	40201.709161	31.050970
500.112539	40272.622017	31.055988
500.834690	40338.955779	31.061005
501.545680	40402.693843	31.066023
501.927975	40479.551138	31.071040
502.673163	40522.826763	31.076058
503.406503	40590.778877	31.081076
503.342693	40654.251235	31.086093
504.345744	40718.983815	31.091111
504.738134	40777.037236	31.096128
505.012626	40840.997288	31.101146
505.389052	40911.727342	31.106164
505.793231	40973.993456	31.111181
506.867321	41039.072130	31.116199
507.331298	41113.260748	31.121216
507.510639	41169.137827	31.126234
508.217466	41232.352319	31.131252
508.146528	41306.465930	31.136269
508.926347	41371.528103	31.141287
509.067103	41447.965332	31.146304
509.802695	41511.911538	31.151322
509.918165	41587.797952	31.156340
510.864144	41667.575443	31.161357
511.490860	41732.080195	31.166375
511.515909	41805.662264	31.171392
512.310592	41868.703445	31.176410
512.583480	41943.593053	31.181428
512.777405	42021.207661	31.186445
513.643322	42103.001651	31.191463
514.235634	42176.788241	31.196480
514.759616	42246.785632	31.201498
515.002926	42318.515384	31.206516
515.513239	42393.392858	31.211533
516.309958	42454.339581	31.216551
516.461340	42531.164686	31.221568
517.008328	42592.547721	31.226586
517.542361	42661.086559	31.231604
517.846191	42734.215892	31.236621
518.036441	42808.134558	31.241639
518.463076	42902.490164	31.246656
519.382615	42970.265639	31.251674
519.657155	43052.912871	31.256692
520.017615	43133.655269	31.261709
521.425641	43197.723563	31.266727
521.587844	43283.755699	31.271744
521.868742	43370.210606	31.276762
522.537189	43455.051816	31.281780
522.996057	43528.101854	31.286797
523.924152	43607.268762	31.291815
524.421481	43679.473274	31.296832
524.899636	43751.141378	31.301850
525.399893	43826.111555	31.306868
525.814165	43905.642430	31.311885
526.702246	43974.923237	31.316903
527.061718	44058.470165	31.321920
527.891715	44130.031104	31.326938
528.147821	44206.883745	31.331956
528.234188	44293.943369	31.336973
528.793885	44367.488355	31.341991
529.260484	44456.686473	31.347008
530.157023	44538.615620	31.352026
530.706511	44619.001752	31.357044
530.969278	44705.604784	31.362061
531.797392	44781.171887	31.367079
532.315022	44871.926392	31.372096
533.287923	44949.197274	31.377114
533.401279	45030.402328	31.382132
534.049986	45104.282820	31.387149
534.613628	45176.842120	31.392167
535.039484	45261.097023	31.397184
535.467714	45343.195463	31.402202
536.521317	45413.717217	31.407220
536.765282	45502.110940	31.412237
537.545813	45592.553991	31.417255
538.031254	45665.083900	31.422272
538.195136	45744.127219	31.427290
538.537867	45834.530084	31.432308
538.974330	45908.009929	31.437325
539.859095	45994.430943	31.442343
540.400551	46086.721919	31.447360
540.684294	46174.847019	31.452378
541.450321	46256.423205	31.457396
541.528032	46347.977433	31.462413
542.188134	46432.640962	31.467431
543.005237	46516.186438	31.472448
543.315506	46600.122281	31.477466
543.999135	46688.344773	31.482484
544.865503	46767.809995	31.487501
545.229363	46851.340253	31.492519
545.744704	46937.479292	31.497536
546.506492	47034.155995	31.502554
547.014364	47106.021508	31.507572
547.334845	47195.935690	31.512589
548.113723	47277.769952	31.517607
548.456459	47369.642184	31.522624
549.009622	47454.163770	31.527642
549.759035	47540.500569	31.532660
550.581771	47627.574028	31.537677
551.121400	47688.779264	31.542695
551.535520	47782.732122	31.547712
552.218396	47856.475698	31.552730
552.846665	47920.651112	31.557748
552.894115	47997.117967	31.562765
553.467509	48073.409843	31.567783
553.963810	48157.085047	31.572800
554.412043	48228.162599	31.577818
555.219182	48322.106900	31.582836
555.303527	48404.749160	31.587853
556.193273	48481.849360	31.592871
556.577006	48573.550138	31.597888
557.024240	48665.032451	31.602906
557.380685	48743.207055	31.607924
557.966889	48830.195637	31.612941
558.708316	48934.300173	31.617959
559.021921	49035.314844	31.622976
559.350145	49122.660009	31.627994
560.265374	49220.702557	31.633012
560.854276	49315.619418	31.638029
561.270655	49403.794494	31.643047
561.937185	49494.372963	31.648064
562.384215	49583.150144	31.653082
563.266256	49675.348686	31.658100
563.876671	49766.168252	31.663117
564.706119	49852.309704	31.668135
565.103397	49948.483538	31.673152
565.600788	50040.968443	31.678170
566.304565	50130.021570	31.683188
567.053754	50217.150623	31.688205
567.520820	50308.713340	31.693223
567.674203	50396.525875	31.698240
568.369861	50485.414613	31.703258
568.759973	50574.543722	31.708276
569.379196	50683.412111	31.713293
570.321338	50767.331480	31.718311
570.586980	50866.339324	31.723328
571.193188	50957.019955	31.728346
572.297893	51037.850149	31.733364
572.571099	51138.364640	31.738381
573.412258	51225.555726	31.743399
574.067668	51325.546957	31.748416
574.626902	51420.220169	31.753434
575.514473	51499.351086	31.758452
575.332027	51590.556596	31.763469
576.189319	51672.368357	31.768487
576.690860	51766.945416	31.773504
577.233096	51853.787604	31.778522
577.884886	51952.408781	31.783540
578.330000	52046.885987	31.788557
579.221739	52132.215664	31.793575
579.875996	52236.873682	31.798592
580.235259	52327.828961	31.803610
581.083045	52409.367470	31.808628
581.271778	52492.929232	31.813645
582.024163	52585.412679	31.818663
582.594024	52669.632397	31.823680
583.035148	52762.976686	31.828698
583.566369	52869.585162	31.833716
584.369538	52956.187055	31.838733
584.593881	53045.007514	31.843751
585.685674	53139.629615	31.848768
586.371687	53244.382589	31.853786
587.043504	53312.883561	31.858804
587.587077	53402.720551	31.863821
588.236778	53494.656735	31.868839
589.025878	53569.810355	31.873856
589.355736	53650.788941	31.878874
590.086750	53746.591765	31.883892
590.443559	53833.144942	31.888909
591.343444	53906.241028	31.893927
591.580710	53991.342680	31.898944
591.927652	54078.290259	31.903962
592.748778	54152.954391	31.908980
592.948287	54242.940528	31.913997
593.685643	54339.402247	31.919015
594.587319	54412.853724	31.924032
594.714810	54501.065052	31.929050
595.552108	54589.336441	31.934068
595.573976	54677.559692	31.939085
596.247921	54772.182927	31.944103
597.034351	54876.410029	31.949120
597.338988	54972.908435	31.954138
598.002343	55061.987776	31.959156
598.716971	55159.158571	31.964173
599.428893	55251.313876	31.969191
600.293496	55338.421638	31.974208
601.002311	55435.935934	31.979226
601.560662	55536.268120	31.984244
601.885759	55630.908890	31.989261
602.202846	55720.402219	31.994279
603.453014	55816.906559	31.999296
603.847187	55913.154708	32.004314
605.156989	55987.978899	32.009332
605.376847	56086.531218	32.014349
606.054486	56174.507564	32.019367
606.287069	56267.384938	32.024384
606.903186	56376.885946	32.029402
607.589359	56464.103982	32.034420
608.246183	56563.629034	32.039437
608.846600	56657.881754	32.044455
609.640654	56756.260443	32.049472
610.254776	56840.800409	32.054490
610.726431	56934.108995	32.059508
611.173477	57031.099439	32.064525
611.893822	57130.269335	32.069543
612.719338	57231.096771	32.074560
613.293384	57328.844879	32.079578
613.770211	57427.456217	32.084596
614.529470	57516.019002	32.089613
614.715116	57617.939793	32.094631
615.315137	57707.231102	32.099648
615.857648	57820.126431	32.104666
616.851718	57921.036954	32.109684
617.071681	58030.985340	32.114701
617.696778	58130.472948	32.119719
618.592463	58227.944879	32.124736
618.876389	58341.334511	32.129754
619.666201	58441.422038	32.134772
620.012067	58549.475770	32.139789
620.716418	58656.459840	32.144807
621.713096	58764.672647	32.149824
622.069429	58871.279333	32.154842
622.708219	58965.738873	32.159860
623.447358	59069.490355	32.164877
624.139685	59169.111059	32.169895
624.780217	59275.508663	32.174912
625.285479	59376.873796	32.179930
626.187444	59482.666914	32.184948
626.930163	59592.385891	32.189965
627.437077	59683.255964	32.194983
628.140145	59775.433754	32.200000
628.871227	59878.950624	32.205018
629.343460	59972.759927	32.210036
630.103154	60074.870172	32.215053
630.498406	60180.965519	32.220071
631.452563	60273.192597	32.225088
631.836749	60364.048101	32.230106
632.604811	60456.540577	32.235124
633.479733	60544.952333	32.240141
633.817024	60636.600440	32.245159
634.455159	60728.287752	32.250176
635.000690	60816.710865	32.255194
635.506556	60909.533108	32.260212
636.282382	61006.937236	32.265229
637.446366	61105.276251	32.270247
637.963617	61182.943084	32.275264
638.617864	61276.336567	32.280282
638.971672	61374.671662	32.285300
639.218576	61462.110463	32.290317
639.806067	61565.899864	32.295335
640.657538	61661.095323	32.300352
641.007918	61763.831549	32.305370
641.746365	61873.576286	32.310388
642.270075	61956.206220	32.315405
642.631495	62072.315368	32.320423
643.473566	62183.858527	32.325440
643.723466	62294.463596	32.330458
644.750960	62404.883962	32.335476
645.395538	62513.295141	32.340493
646.173617	62607.685533	32.345511
647.094642	62716.968574	32.350528
647.949490	62818.476525	32.355546
649.028801	62910.296773	32.360564
649.855399	63008.201429	32.365581
650.311047	63099.392367	32.370599
650.906858	63209.054096	32.375616
651.410008	63305.275481	32.380634
652.153257	63397.899238	32.385652
652.947834	63506.727037	32.390669
653.373600	63607.829417	32.395687
654.029845	63700.702774	32.400704
654.143601	63817.033408	32.405722
655.028862	63913.504254	32.410740
655.996292	64020.277312	32.415757
656.457091	64122.583693	32.420775
656.974107	64212.075503	32.425792
657.538950	64328.517838	32.430810
657.917972	64436.913542	32.435828
658.540366	64549.409767	32.440845
659.617675	64658.468778	32.445863
659.884727	64779.956331	32.450880
660.395409	64891.550023	32.455898
661.272954	64998.968781	32.460916
661.892778	65118.743975	32.465933
662.347624	65248.831446	32.470951
662.813364	65360.333958	32.475968
663.609012	65470.189667	32.480986
664.488939	65585.234345	32.486004
665.193931	65707.268176	32.491021
665.858992	65815.042329	32.496039
666.909625	65923.455025	32.501056
667.299860	66058.766968	32.506074
668.826738	66159.010994	32.511092
670.079473	66250.861777	32.516109
670.788842	66345.969715	32.521127
671.790366	66425.415968	32.526144
672.479254	66526.912735	32.531162
672.983423	66622.188576	32.536180
673.717063	66711.762901	32.541197
673.955106	66797.999519	32.546215
674.755570	66879.193844	32.551232
675.238201	66984.380756	32.556250
675.643052	67080.452650	32.561268
676.481164	67169.303671	32.566285
676.862700	67266.284264	32.571303
677.731712	67360.681413	32.576320
678.252559	67458.095052	32.581338
678.767619	67545.705075	32.586356
679.911082	67627.920367	32.591373
680.544739	67727.820052	32.596391
681.117915	67803.922214	32.601408
681.609086	67908.530763	32.606426
682.088271	67999.119881	32.611444
682.964536	68094.581224	32.616461
683.404765	68183.679281	32.621479
684.146809	68290.701217	32.626496
684.573962	68389.209395	32.631514
685.019121	68505.429387	32.636532
685.609086	68608.798638	32.641549
686.299039	68710.381698	32.646567
686.774226	68809.294848	32.651584
687.343689	68931.249797	32.656602
687.926939	69048.809249	32.661620
688.870296	69173.808052	32.666637
689.446601	69299.178005	32.671655
690.707915	69386.293132	32.676672
691.495703	69498.358849	32.681690
692.413961	69611.781889	32.686708
693.406482	69716.133282	32.691725
693.793777	69829.120416	32.696743
694.641002	69941.785622	32.701760
695.283884	70041.416581	32.706778
695.809314	70153.921094	32.711796
696.760917	70257.693921	32.716813
696.925262	70359.099846	32.721831
697.427079	70466.077652	32.726848
698.170504	70591.933473	32.731866
698.771853	70710.801638	32.736884
699.562860	70822.861185	32.741901
699.804632	70943.712142	32.746919
700.795551	71062.416772	32.751936
701.827752	71182.955190	32.756954
702.073691	71317.034942	32.761972
702.962237	71439.545979	32.766989
703.476815	71562.132124	32.772007
704.446996	71679.787685	32.777024
704.765835	71815.515146	32.782042
705.312598	71927.298359	32.787060
706.207923	72065.031452	32.792077
706.695141	72198.343404	32.797095
707.620519	72316.016186	32.802112
708.707352	72458.582697	32.807130
708.961248	72588.476811	32.812148
709.953703	72700.304269	32.817165
710.729983	72840.534404	32.822183
711.961050	72970.383272	32.827200
712.799900	73079.885784	32.832218
713.286604	73201.360337	32.837236
714.524863	73313.618327	32.842253
714.934466	73425.406692	32.847271
715.838058	73530.847447	32.852288
716.662006	73650.308545	32.857306
717.255944	73773.159792	32.862324
718.046145	73873.460894	32.867341
718.686092	73987.307247	32.872359
719.194882	74116.668902	32.877376
719.855773	74224.094493	32.882394
720.798944	74353.689368	32.887412
721.288596	74459.051237	32.892429
721.981764	74588.372610	32.897447
722.619776	74709.501806	32.902464
723.316251	74817.967900	32.907482
723.539487	74937.187481	32.912500
724.720757	75043.671138	32.917517
725.686301	75158.955999	32.922535
726.561025	75265.953020	32.927552
727.365808	75366.018301	32.932570
727.900314	75480.648781	32.937588
728.823785	75581.232997	32.942605
729.590336	75697.122739	32.947623
729.903847	75797.777061	32.952640
730.715570	75911.219345	32.957658
731.338813	76039.409871	32.962676
731.591231	76144.547123	32.967693
732.306409	76269.586971	32.972711
733.261794	76383.842790	32.977728
734.457040	76491.849050	32.982746
734.705295	76611.472068	32.987764
736.053807	76728.004795	32.992781
736.639464	76848.471457	32.997799
736.862376	76969.662757	33.002816
738.061553	77090.655557	33.007834
738.400053	77206.655588	33.012852
739.502938	77321.884890	33.017869
740.078203	77455.556077	33.022887
740.786316	77580.952407	33.027904
741.489752	77691.177198	33.032922
742.619403	77815.379447	33.037940
743.579869	77944.942139	33.042957
743.759700	78049.898083	33.047975
744.447603	78172.467583	33.052992
745.496749	78291.341292	33.058010
746.470818	78406.888472	33.063028
747.445511	78528.387944	33.068045
748.064552	78664.658768	33.073063
748.752533	78784.739589	33.078080
749.841354	78888.714489	33.083098
750.361012	79012.518177	33.088116
751.210477	79134.781683	33.093133
751.727161	79257.012263	33.098151
752.429257	79369.187444	33.103168
753.194924	79497.336568	33.108186
753.682765	79616.506139	33.113204
754.485648	79733.771007	33.118221
755.030532	79871.921101	33.123239
756.064416	80003.299041	33.128256
756.881120	80127.996021	33.133274
757.253043	80266.316270	33.138292
757.876981	80376.010856	33.143309
758.641441	80508.758279	33.148327
759.487111	80651.582353	33.153344
760.581934	80780.064001	33.158362
760.977147	80915.310160	33.163380
762.054415	81039.330288	33.168397
762.764623	81171.008892	33.173415
763.393330	81299.627411	33.178432
764.318972	81421.448019	33.183450
764.906375	81564.598871	33.188468
765.975399	81688.497417	33.193485
767.094572	81818.284094	33.198503
767.756065	81950.601556	33.203520
768.389593	82073.871953	33.208538
769.149927	82207.667524	33.213556
769.944460	82336.112735	33.218573
770.748044	82462.703639	33.223591
771.473968	82592.584999	33.228608
772.540897	82707.715159	33.233626
772.618560	82847.225868	33.238644
773.554531	82969.824897	33.243661
774.581478	83099.096409	33.248679
774.947461	83221.822550	33.253696
775.802189	83344.981076	33.258714
776.175412	83477.089327	33.263732
776.907648	83611.707572	33.268749
777.992593	83731.160859	33.273767
778.596492	83865.909344	33.278784
779.488423	83983.839515	33.283802
779.549776	84122.120713	33.288820
780.775369	84243.343859	33.293837
781.771569	84372.817456	33.298855
782.586216	84510.464148	33.303872
783.779715	84629.404393	33.308890
784.786690	84760.124751	33.313908
785.361075	84885.001781	33.318925
786.140418	85008.719477	33.323943
786.782933	85135.800989	33.328960
787.695665	85257.859353	33.333978
788.341277	85399.645401	33.338996
789.037470	85526.644281	33.344013
789.765921	85659.566888	33.349031
790.434058	85802.167865	33.354048
791.187821	85932.481140	33.359066
791.922952	86074.205928	33.364084
792.570961	86208.865936	33.369101
793.207408	86343.104717	33.374119
794.215251	86503.452172	33.379136
795.175525	86632.058574	33.384154
795.561682	86783.589240	33.389172
796.139197	86936.158608	33.394189
797.285838	87081.877393	33.399207
797.647030	87233.750459	33.404224
798.962933	87367.541274	33.409242
799.653542	87525.992982	33.414260
800.605676	87679.005218	33.419277
801.324645	87823.502116	33.424295
802.381396	87973.126419	33.429312
803.286088	88118.891627	33.434330
803.922416	88279.983366	33.439348
805.029979	88416.902488	33.444365
805.982398	88551.430831	33.449383
806.903745	88711.092687	33.454400
807.594011	88843.204481	33.459418
808.507853	88974.995344	33.464436
809.109879	89125.442434	33.469453
810.123331	89259.034542	33.474471
811.009412	89419.130990	33.479488
811.582157	89540.730024	33.484506
812.626601	89685.077036	33.489524
813.262793	89837.788459	33.494541
814.464038	89972.125615	33.499559
815.021377	90121.573921	33.504576
816.296231	90258.501419	33.509594
816.950402	90391.849168	33.514612
817.741046	90526.586332	33.519629
818.207961	90676.850424	33.524647
818.711800	90832.387208	33.529664
819.705566	90971.067551	33.534682
820.468258	91124.785223	33.539700
821.078495	91271.365235	33.544717
821.927323	91414.293173	33.549735
822.818604	91576.238557	33.554752
823.776036	91719.694642	33.559770
824.571228	91876.284955	33.564788
825.311245	92025.936526	33.569805
826.511014	92168.589513	33.574823
827.069816	92317.500723	33.579840
827.828865	92469.746701	33.584858
828.492802	92615.623567	33.589876
829.155285	92775.247839	33.594893
829.748403	92910.644934	33.599911
830.427060	93055.389157	33.604928
831.401982	93202.230849	33.609946
831.979467	93359.404718	33.614964
832.874170	93515.141165	33.619981
833.731263	93672.739248	33.624999
834.317854	93825.427308	33.630016
835.139149	93967.723045	33.635034
836.322484	94129.789257	33.640052
837.167181	94290.013690	33.645069
837.748170	94444.320524	33.650087
838.913676	94604.905461	33.655104
839.394651	94757.059826	33.660122
840.577877	94930.885046	33.665140
841.409875	95084.584834	33.670157
842.300559	95238.326534	33.675175
842.993876	95403.583582	33.680192
843.930245	95554.635997	33.685210
844.898056	95723.128599	33.690228
845.602428	95884.158868	33.695245
846.776036	96046.828063	33.700263
847.049800	96216.305817	33.705280
847.927236	96368.537642	33.710298
848.686187	96545.147179	33.715316
849.681824	96714.806666	33.720333
850.783865	96873.682548	33.725351
851.331280	97059.876219	33.730368
852.206368	97225.723155	33.735386
853.207181	97390.942756	33.740404
853.945407	97561.973535	33.745421
855.139632	97736.785254	33.750439
855.910322	97902.001943	33.755456
857.009095	98062.696416	33.760474
857.664071	98233.745561	33.765492
858.366726	98412.624934	33.770509
859.575982	98568.404761	33.775527
860.085661	98749.717616	33.780544
860.892511	98917.733096	33.785562
861.663330	99084.565522	33.790580
862.579495	99276.836449	33.795597
863.695836	99456.034802	33.800615
864.624334	99626.351934	33.805632
865.618284	99794.810858	33.810650
866.305971	99969.500248	33.815668
867.202518	100146.897577	33.820685
868.016712	100320.599905	33.825703
868.901523	100496.640508	33.830720
870.094292	100667.756707	33.835738
870.924282	100846.005609	33.840756
871.983836	101022.375546	33.845773
872.629314	101184.361379	33.850791
873.607172	101357.328387	33.855808
874.379676	101538.788825	33.860826
875.394376	101705.889523	33.865844
876.211147	101893.796614	33.870861
877.424116	102055.960199	33.875879
878.124141	102225.192898	33.880896
878.782160	102388.102342	33.885914
879.576728	102566.635046	33.890932
880.194386	102744.698024	33.895949
881.249355	102918.580924	33.900967
882.175835	103107.523495	33.905984
882.784475	103283.236380	33.911002
883.949937	103459.270076	33.916020
884.963705	103644.080318	33.921037
885.680526	103816.220604	33.926055
886.230444	104002.534622	33.931072
887.266043	104183.229506	33.936090
888.150206	104346.569885	33.941108
889.040212	104511.005736	33.946125
890.405671	104677.402987	33.951143
891.050615	104846.104782	33.956160
891.740852	105016.807420	33.961178
892.757669	105191.712356	33.966196
893.482624	105361.050138	33.971213
894.514219	105526.729105	33.976231
894.975027	105702.216836	33.981248
895.938368	105895.010891	33.986266
896.709147	106059.558514	33.991284
897.332940	106245.521773	33.996301
898.571776	106434.259659	34.001319
899.341630	106625.482626	34.006336
900.201725	106795.985182	34.011354
901.082006	106980.163547	34.016372
901.616855	107183.878923	34.021389
902.881027	107356.332110	34.026407
903.818050	107552.688865	34.031424
904.767297	107749.614994	34.036442
905.298280	107926.182496	34.041460
906.279467	108137.582680	34.046477
907.423826	108336.824050	34.051495
908.388338	108526.774728	34.056512
909.093924	108712.437848	34.061530
910.076393	108920.576290	34.066548
910.731204	109113.356084	34.071565
912.046245	109302.659110	34.076583
912.883090	109516.766569	34.081600
913.668664	109718.129380	34.086618
914.720175	109917.195199	34.091636
915.554386	110112.549132	34.096653
916.802923	110330.926991	34.101671
917.603712	110520.817498	34.106688
918.305334	110711.359044	34.111706
919.204551	110903.262645	34.116724
920.076150	111119.543105	34.121741
922.212712	111312.537325	34.126759
923.301176	111507.504683	34.131776
923.818344	111702.073748	34.136794
925.062629	111887.555792	34.141812
925.952909	112078.633140	34.146829
927.220674	112247.811000	34.151847
927.965744	112443.639794	34.156864
928.385923	112641.664441	34.161882
929.584477	112813.188049	34.166900
930.655297	113003.304643	34.171917
931.490857	113202.696205	34.176935
932.117732	113388.252353	34.181952
933.031341	113589.597350	34.186970
934.236439	113776.922836	34.191988
935.264311	113973.070537	34.197005
936.189721	114174.126480	34.202023
936.899709	114374.193318	34.207040
937.638417	114567.314570	34.212058
938.571691	114760.810432	34.217076
939.044538	114970.827482	34.222093
940.485233	115153.689368	34.227111
940.983501	115368.101242	34.232128
941.926703	115578.665980	34.237146
942.784296	115778.059750	34.242164
943.821985	115991.183788	34.247181
944.676910	116208.191043	34.252199
945.704491	116421.497386	34.257216
946.686474	116626.679161	34.262234
947.613245	116829.641727	34.267252
948.560715	117047.121608	34.272269
949.298770	117242.934683	34.277287
950.602211	117435.196938	34.282304
951.406678	117635.537517	34.287322
952.361371	117821.182993	34.292340
953.199691	118019.404822	34.297357
953.872295	118233.188874	34.302375
954.937932	118427.511648	34.307392
955.614732	118639.283499	34.312410
956.895849	118847.814904	34.317428
957.424985	119055.977836	34.322445
958.644258	119256.147280	34.327463
959.465458	119465.050532	34.332480
960.325241	119682.628356	34.337498
961.474532	119895.117052	34.342516
962.250982	120123.089337	34.347533
963.543379	120329.779684	34.352551
964.122052	120533.345551	34.357568
965.156643	120760.874769	34.362586
966.350944	120981.017399	34.367604
967.038158	121186.242533	34.372621
967.873290	121422.717825	34.377639
968.932172	121646.930044	34.382656
969.751697	121869.776949	34.387674
970.960046	122107.273257	34.392692
971.871743	122326.028114	34.397709
972.938680	122541.933129	34.402727
973.877543	122783.711832	34.407744
974.710953	123012.597015	34.412762
976.078540	123245.577621	34.417780
976.887617	123465.232269	34.422797
977.930979	123691.249443	34.427815
978.803755	123925.254854	34.432832
979.483170	124164.375758	34.437850
980.975869	124391.781434	34.442868
981.833932	124632.790187	34.447885
982.833148	124861.827007	34.452903
983.837127	125095.528469	34.457920
984.980988	125339.321818	34.462938
986.095518	125562.439278	34.467956
987.241672	125799.658583	34.472973
987.806300	126030.524992	34.477991
989.043150	126266.871208	34.483008
989.814537	126498.112609	34.488026
990.480412	126719.094814	34.493044
991.782166	126965.828218	34.498061
993.154785	127200.904599	34.503079
994.146982	127430.836586	34.508096
995.219308	127677.423529	34.513114
996.113390	127908.439939	34.518132
997.157055	128143.768009	34.523149
998.420545	128383.915890	34.528167
999.397604	128600.183489	34.533184
1000.119673	128856.508382	34.538202
1001.207752	129069.833120	34.543220
1002.381776	129306.010440	34.548237
1003.178284	129543.912300	34.553255
1004.329810	129767.434655	34.558272
1004.807951	130014.987642	34.563290
1006.122282	130254.102312	34.568308
1007.208970	130491.266384	34.573325
1007.708221	130729.315114	34.578343
1009.316047	130967.575575	34.583360
1010.131057	131216.578179	34.588378
1011.129648	131452.014850	34.593396
1012.266398	131691.689526	34.598413
1013.177353	131923.709066	34.603431
1014.404538	132160.203415	34.608448
1015.002476	132408.021706	34.613466
1016.375704	132632.656059	34.618484
1017.269702	132868.830422	34.623501
1017.928457	133094.080365	34.628519
1019.292309	133317.719680	34.633536
1020.115765	133549.689497	34.638554
1021.170917	133782.738284	34.643572
1022.190520	134014.463586	34.648589
1022.766702	134243.956595	34.653607
1023.822839	134488.863126	34.658624
1024.874996	134724.809570	34.663642
1026.145337	134957.932768	34.668660
1026.944484	135195.509051	34.673677
1027.779217	135442.639835	34.678695
1028.853118	135687.729997	34.683712
1030.064548	135942.129890	34.688730
1031.292458	136172.378365	34.693748
1032.156226	136418.244011	34.698765
1033.092435	136675.915172	34.703783
1034.112644	136909.106320	34.708800
1035.034355	137169.027718	34.713818
1036.524381	137418.309249	34.718836
1037.401405	137668.454550	34.723853
1038.109423	137923.612176	34.728871
1039.847480	138169.688881	34.733888
1040.325445	138428.805965	34.738906
1041.382157	138680.032254	34.743924
1042.672878	138937.954131	34.748941
1043.631603	139185.536295	34.753959
1044.705240	139434.508663	34.758976
1045.821412	139702.418084	34.763994
1046.800794	139960.703528	34.769012
1048.172914	140213.169822	34.774029
1048.969387	140480.922670	34.779047
1050.233447	140734.412353	34.784064
1050.635159	140986.917832	34.789082
1052.004077	141252.959317	34.794100
1053.169357	141522.789647	34.799117
1054.056607	141778.555560	34.804135
1055.315761	142036.341468	34.809152
1056.073838	142306.967954	34.814170
1057.528156	142570.330145	34.819188
1058.520563	142825.465186	34.824205
1059.688999	143084.820895	34.829223
1061.148982	143349.608276	34.834240
1062.347179	143618.156232	34.839258
1063.391293	143864.579015	34.844276
1064.551388	144117.134439	34.849293
1065.781914	144383.933056	34.854311
1066.851926	144625.183252	34.859328
1067.936686	144879.252940	34.864346
1069.060613	145135.384982	34.869364
1070.269789	145386.039320	34.874381
1071.151823	145651.167804	34.879399
1072.133820	145898.553527	34.884416
1073.121227	146156.211885	34.889434
1074.273384	146415.785159	34.894452
1075.414985	146664.481409	34.899469
1076.219388	146919.918214	34.904487
1077.278087	147174.503241	34.909504
1078.524032	147441.309680	34.914522
1079.505011	147697.623278	34.919540
1080.882853	147951.463630	34.924557
1081.574648	148216.807425	34.929575
1083.252574	148465.148605	34.934592
1083.834121	148729.005189	34.939610
1084.915245	148985.260651	34.944628
1086.262053	149243.262265	34.949645
1086.829524	149513.379239	34.954663
1088.038202	149765.028083	34.959680
1089.173347	150010.920214	34.964698
1090.105387	150267.982909	34.969716
1091.697006	150518.419573	34.974733
1092.161135	150760.381676	34.979751
1093.162178	151010.208924	34.984768
1094.421876	151270.686942	34.989786
1095.204414	151538.563709	34.994804
1096.222359	151780.796160	34.999821
1096.860072	152045.618457	35.004839
1098.162052	152301.644858	35.009856
1099.569356	152582.007866	35.014874
1100.288582	152860.292294	35.019892
1101.429801	153107.091716	35.024909
1102.275419	153395.049520	35.029927
1103.197901	153673.560050	35.034944
1104.345582	153951.946656	35.039962
1105.211372	154225.105277	35.044980
1106.929248	154508.310529	35.049997
1107.750069	154801.546952	35.055015
1108.853696	155097.935371	35.060032
1110.189541	155361.346361	35.065050
1111.031660	155666.496491	35.070068
1112.579577	155962.640617	35.075085
1113.525034	156244.984042	35.080103
1114.338523	156535.748616	35.085120
1115.376104	156828.089338	35.090138
1116.285795	157120.022063	35.095156
1117.785428	157412.747526	35.100173
1118.836090	157718.386650	35.105191
1120.052482	158007.915884	35.110208
1121.345102	158301.100713	35.115226
1122.192575	158618.806024	35.120244
1123.793651	158918.896105	35.125261
1124.356388	159215.569809	35.130279
1125.671490	159512.730423	35.135296
1127.123611	159814.577054	35.140314
1127.984389	160106.324084	35.145332
1129.458031	160407.232831	35.150349
1130.529748	160714.515148	35.155367
1131.635371	160999.821701	35.160384
1133.058326	161313.520508	35.165402
1134.137521	161618.106209	35.170420
1135.514552	161907.890636	35.175437
1136.638223	162214.490557	35.180455
1137.877135	162509.325886	35.185472
1139.098813	162805.802745	35.190490
1139.705936	163112.900551	35.195508
1141.203855	163415.438519	35.200525
1141.963702	163708.826297	35.205543
1143.313922	164004.427724	35.210560
1144.533260	164314.160996	35.215578
1145.525986	164616.778312	35.220596
1147.118072	164920.225032	35.225613
1148.278315	165216.690968	35.230631
1149.239875	165521.768551	35.235648
1150.470491	165809.358380	35.240666
1151.885161	166117.524633	35.245684
1153.202115	166409.075484	35.250701
1154.013645	166707.055688	35.255719
1155.116323	166999.051898	35.260736
1156.324033	167305.370265	35.265754
1157.025189	167608.006013	35.270772
1158.267771	167915.959679	35.275789
1159.457631	168220.219210	35.280807
1161.084912	168525.753613	35.285824
1162.277345	168826.311877	35.290842
1163.063608	169127.091487	35.295860
1163.968498	169426.978029	35.300877
1164.844747	169728.432032	35.305895
1166.075266	170015.986037	35.310912
1167.354940	170320.549643	35.315930
1168.219142	170622.303477	35.320948
1169.872623	170909.983705	35.325965
1170.903653	171211.802752	35.330983
1171.931756	171516.060625	35.336000
1173.409616	171811.465245	35.341018
1173.983254	172106.208902	35.346036
1175.638533	172417.932145	35.351053
1176.425217	172716.438708	35.356071
1177.505766	173026.509757	35.361088
1178.850245	173331.273051	35.366106
1179.647279	173665.125045	35.371124
1181.036584	173963.121361	35.376141
1182.343770	174280.510805	35.381159
1183.517959	174606.033326	35.386176
1184.747303	174919.163339	35.391194
1185.849586	175243.636129	35.396212
1187.065333	175556.036539	35.401229
1188.618129	175864.411240	35.406247
1189.998369	176182.626193	35.411264
1191.310111	176501.438322	35.416282
1192.199339	176817.251141	35.421300
1193.582007	177125.496998	35.426317
1194.720081	177448.303533	35.431335
1195.506346	177780.320447	35.436352
1196.623917	178102.893546	35.441370
1198.025469	178421.716071	35.446388
1199.088144	178749.264678	35.451405
1200.203040	179092.645554	35.456423
1201.576536	179428.891625	35.461440
1202.721737	179747.434969	35.466458
1203.977571	180077.650978	35.471476
1205.391527	180419.646256	35.476493
1206.387581	180743.563671	35.481511
1207.430709	181073.123220	35.486528
1208.758475	181417.081261	35.491546
1209.840554	181759.305282	35.496564
1210.957327	182087.133068	35.501581
1212.444924	182428.279215	35.506599
1213.413521	182775.567447	35.511616
1214.969179	183113.724172	35.516634
1216.005847	183458.721081	35.521652
1217.184643	183792.349731	35.526669
1218.750050	184147.049739	35.531687
1219.571158	184489.334653	35.536704
1221.126073	184818.122532	35.541722
1222.108416	185169.993551	35.546740
1223.764101	185509.786355	35.551757
1225.014956	185855.004530	35.556775
1226.262157	186201.520185	35.561792
1227.616130	186539.160626	35.566810
1228.622129	186881.214337	35.571828
1229.773488	187225.416720	35.576845
1231.101109	187572.270438	35.581863
1232.744387	187913.755673	35.586880
1233.903342	188244.013033	35.591898
1234.912303	188590.976431	35.596916
1236.238592	188928.839014	35.601933
1237.682426	189278.552832	35.606951
1238.661393	189617.098818	35.611968
1239.820335	189957.901992	35.616986
1240.611727	190316.425126	35.622004
1241.745958	190656.614496	35.627021
1243.024050	191013.055943	35.632039
1244.073882	191377.509180	35.637056
1245.692206	191717.193212	35.642074
1246.480989	192061.814570	35.647092
1247.649099	192409.726639	35.652109
1249.278586	192748.754620	35.657127
1250.205647	193091.480315	35.662144
1251.068177	193439.309149	35.667162
1251.844877	193794.859822	35.672180
1253.869531	194152.085414	35.677197
1255.101673	194497.536140	35.682215
1256.079003	194874.730051	35.687232
1257.164461	195231.012460	35.692250
1258.003631	195597.277788	35.697268
1259.321389	195959.835457	35.702285
1260.741533	196341.052967	35.707303
1261.812161	196723.523814	35.712320
1262.960335	197086.471387	35.717338
1264.109742	197470.507925	35.722356
1265.486974	197839.439577	35.727373
1266.679649	198225.453954	35.732391
1268.187405	198615.963654	35.737408
1269.647887	198985.510130	35.742426
1270.711762	199375.640549	35.747444
1271.802284	199769.971194	35.752461
1273.671267	200155.136158	35.757479
1274.658786	200544.524234	35.762496
1276.070458	200939.557784	35.767514
1277.287150	201314.489676	35.772532
1279.032284	201705.917683	35.777549
1280.425787	202082.221157	35.782567
1281.501285	202482.207114	35.787584
1283.119201	202863.023061	35.792602
1284.178439	203263.168502	35.797620
1285.432335	203656.834200	35.802637
1286.763642	204048.597486	35.807655
1288.156908	204454.039754	35.812672
1289.483054	204823.246002	35.817690
1290.369327	205219.075858	35.822708
1291.670731	205616.604202	35.827725
1293.037291	206021.843704	35.832743
1294.105804	206423.541326	35.837760
1295.808268	206822.330397	35.842778
1297.005431	207222.119165	35.847796
1298.374282	207613.285640	35.852813
1300.001221	208014.747141	35.857831
1300.898385	208420.318153	35.862848
1302.502624	208817.279968	35.867866
1303.919181	209208.471992	35.872884
1305.063075	209626.515570	35.877901
1306.868601	210019.031422	35.882919
1308.388391	210416.091341	35.887936
1309.400194	210801.872529	35.892954
1311.083352	211209.956424	35.897972
1312.382360	211589.573552	35.902989
1314.505829	211969.221418	35.908007
1315.675423	212364.951750	35.913024
1316.627538	212733.545948	35.918042
1317.971105	213126.762302	35.923060
1319.137697	213524.276260	35.928077
1320.520194	213892.271082	35.933095
1321.736185	214293.996229	35.938112
1323.127492	214687.592723	35.943130
1324.110023	215076.229856	35.948148
1325.519963	215455.782224	35.953165
1326.731428	215865.566037	35.958183
1327.844660	216253.094596	35.963200
1328.882846	216655.342194	35.968218
1330.391855	217056.345555	35.973236
1332.172565	217464.594875	35.978253
1333.336032	217851.131294	35.983271
1334.505784	218249.224199	35.988288
1335.914022	218626.021432	35.993306
1336.995541	219004.042355	35.998324
1337.871933	219437.136061	36.003341
1339.607978	219852.031727	36.008359
1340.468120	220263.670312	36.013376
1341.674601	220649.270937	36.018394
1343.476665	221048.312082	36.023412
1344.253435	221446.863626	36.028429
1346.023732	221842.433483	36.033447
1347.338305	222249.661851	36.038464
1348.484135	222646.455325	36.043482
1349.884511	223060.885889	36.048500
1351.255224	223474.814954	36.053517
1352.679321	223874.056098	36.058535
1353.601025	224293.675539	36.063552
1355.209003	224702.439397	36.068570
1356.592527	225122.214300	36.073588
1357.895395	225535.044598	36.078605
1359.696503	225956.353786	36.083623
1360.860541	226386.761098	36.088640
1362.072746	226807.891116	36.093658
1362.801434	227223.362045	36.098676
1364.637636	227655.186951	36.103693
1366.330518	228068.596625	36.108711
1367.572067	228521.376075	36.113728
1369.297374	228950.607548	36.118746
1370.648347	229365.576489	36.123764
1371.636622	229806.413349	36.128781
1373.187596	230221.351993	36.133799
1374.239989	230654.535558	36.138816
1375.787490	231092.998319	36.143834
1377.365915	231535.699282	36.148852
1378.460701	231994.534730	36.153869
1379.762943	232421.205384	36.158887
1381.107899	232857.446388	36.163904
1382.794561	233306.180378	36.168922
1384.305026	233746.511651	36.173940
1385.506929	234190.959306	36.178957
1387.567187	234635.596806	36.183975
1388.911835	235073.876345	36.188992
1390.270218	235512.561245	36.194010
1391.969778	235949.412932	36.199028
1392.813642	236376.576625	36.204045
1394.592186	236829.445914	36.209063
1395.676184	237273.540465	36.214080
1397.183823	237711.469836	36.219098
1399.009246	238156.053901	36.224116
1400.199977	238598.305229	36.229133
1401.919997	239021.647502	36.234151
1403.678846	239457.050224	36.239168
1405.309489	239900.298895	36.244186
1406.378483	240324.564342	36.249204
1407.565164	240761.639311	36.254221
1409.238416	241189.871185	36.259239
1410.977005	241625.917024	36.264256
1412.247532	242055.868254	36.269274
1413.803620	242478.558960	36.274292
1414.871391	242911.466574	36.279309
1416.323548	243335.547756	36.284327
1417.897974	243778.508923	36.289344
1419.107145	244200.701163	36.294362
1420.642568	244634.195204	36.299380
1421.569478	245068.501677	36.304397
1423.634346	245507.523782	36.309415
1424.712675	245944.880419	36.314432
1426.101105	246377.461678	36.319450
1428.108993	246808.341000	36.324468
1429.118978	247222.569017	36.329485
1430.499706	247629.547435	36.334503
1431.833952	248046.237928	36.339520
1432.908888	248475.774784	36.344538
1434.484940	248895.525601	36.349556
1435.080889	249314.981415	36.354573
1436.174512	249761.282703	36.359591
1438.393004	250191.877688	36.364608
1439.617603	250609.605432	36.369626
1441.561566	251060.518253	36.374644
1442.380454	251495.511686	36.379661
1443.966239	251939.168456	36.384679
1445.431050	252378.450878	36.389696
1446.604012	252826.571333	36.394714
1448.106417	253275.958775	36.399732
1449.408257	253724.033317	36.404749
1450.809790	254182.151409	36.409767
1452.109940	254655.198242	36.414784
1453.129883	255114.650124	36.419802
1454.792891	255576.053840	36.424820
1456.126094	256065.201781	36.429837
1457.746114	256529.763123	36.434855
1459.199413	256998.721561	36.439872
1460.723792	257469.497506	36.444890
1462.552053	257951.604155	36.449908
1464.038605	258430.007663	36.454925
1465.593119	258905.300884	36.459943
1467.079857	259376.134408	36.464960
1468.518591	259853.123529	36.469978
1469.933614	260335.044853	36.474996
1471.052631	260817.726339	36.480013
1472.970977	261289.936772	36.485031
1474.246292	261768.985161	36.490048
1475.637122	262273.036683	36.495066
1477.279068	262749.636515	36.500084
1478.601948	263252.505081	36.505101
1480.641017	263719.131845	36.510119
1482.053776	264212.459025	36.515136
1483.383330	264707.146102	36.520154
1485.449250	265191.905777	36.525172
1486.815202	265668.880295	36.530189
1488.550257	266153.262178	36.535207
1490.202846	266635.777522	36.540224
1492.000652	267104.118995	36.545242
1493.789239	267575.662446	36.550260
1495.379983	268040.658758	36.555277
1496.588701	268513.745108	36.560295
1498.463109	268989.972783	36.565312
1499.962186	269455.135389	36.570330
1501.876613	269926.579757	36.575348
1502.788041	270398.951222	36.580365
1504.255915	270851.568425	36.585383
1505.927021	271325.871118	36.590400
1507.515165	271807.833200	36.595418
1509.072508	272247.757943	36.600436
1510.497992	272726.621085	36.605453
1512.088876	273199.105556	36.610471
1513.594796	273665.836934	36.615488
1514.675088	274129.259288	36.620506
1516.722622	274612.030618	36.625524
1518.134189	275081.264864	36.630541
1519.830718	275538.029431	36.635559
1521.098691	276015.821090	36.640576
1522.652240	276476.595878	36.645594
1524.162366	276938.774150	36.650612
1525.440522	277433.606591	36.655629
1526.752907	277897.466867	36.660647
1528.629559	278366.770844	36.665664
1529.601904	278830.888605	36.670682
1531.636326	279276.565954	36.675700
1532.684303	279739.170614	36.680717
1534.297915	280186.084038	36.685735
1535.834404	280652.594238	36.690752
1537.253872	281111.222660	36.695770
1538.757836	281569.124835	36.700788
1540.516807	282037.220830	36.705805
1541.727165	282511.756665	36.710823
1543.578214	282960.656803	36.715840
1545.018695	283448.894631	36.720858
1546.638290	283922.851261	36.725876
1547.820212	284395.811969	36.730893
1549.100176	284874.114921	36.735911
1551.007512	285348.680599	36.740928
1552.042810	285822.423558	36.745946
1553.603668	286318.990372	36.750964
1555.238540	286806.246593	36.755981
1556.755086	287295.197297	36.760999
1558.563426	287798.145072	36.766016
1559.776510	288288.184104	36.771034
1561.587320	288776.700444	36.776052
1563.175384	289294.107181	36.781069
1564.409163	289810.173467	36.786087
1565.933538	290305.361427	36.791104
1567.138694	290823.816337	36.796122
1568.853358	291341.169185	36.801140
1570.108225	291851.483810	36.806157
1571.742796	292380.783951	36.811175
1573.296243	292901.687876	36.816192
1574.694030	293437.194942	36.821210
1576.411729	293975.415515	36.826228
1578.048447	294507.144752	36.831245
1579.590820	295042.138376	36.836263
1581.122875	295575.785123	36.841280
1582.539067	296122.021271	36.846298
1584.571944	296644.887326	36.851316
1586.293847	297200.694227	36.856333
1588.095669	297738.096270	36.861351
1589.767633	298261.827100	36.866368
1591.385152	298807.102581	36.871386
1593.084998	299346.647007	36.876404
1594.747362	299877.051389	36.881421
1596.402727	300425.512504	36.886439
1598.503582	300947.203600	36.891456
1599.897459	301488.692230	36.896474
1601.576190	302015.323896	36.901492
1603.153747	302553.728668	36.906509
1604.854889	303099.805596	36.911527
1606.445116	303626.214600	36.916544
1607.547236	304155.266370	36.921562
1609.546693	304700.649963	36.926580
1611.041812	305247.129452	36.931597
1612.268958	305787.707002	36.936615
1614.189148	306332.078098	36.941632
1615.705075	306887.128403	36.946650
1617.216794	307432.423653	36.951668
1618.991140	307968.732649	36.956685
1620.670903	308514.526713	36.961703
1622.353028	309048.380757	36.966720
1623.779815	309602.641063	36.971738
1625.423552	310146.805193	36.976756
1627.084806	310699.622735	36.981773
1628.694045	311256.914706	36.986791
1630.183985	311794.312679	36.991808
1631.716119	312351.863736	36.996826
1633.647628	312911.097216	37.001844
1634.966998	313442.163427	37.006861
1636.451805	313990.847879	37.011879
1638.674055	314514.901221	37.016896
1639.909283	315047.417677	37.021914
1641.665320	315573.546732	37.026932
1643.449675	316110.155029	37.031949
1644.927432	316636.144695	37.036967
1646.668391	317178.618261	37.041984
1648.248762	317717.279877	37.047002
1650.052045	318245.210201	37.052020
1651.188674	318781.600832	37.057037
1652.856467	319335.547625	37.062055
1654.225791	319880.321803	37.067072
1655.675102	320426.348097	37.072090
1657.112843	320995.529472	37.077108
1658.984159	321551.735491	37.082125
1660.469698	322116.252820	37.087143
1662.270901	322689.092435	37.092160
1663.779036	323268.602513	37.097178
1665.323158	323832.613042	37.102196
1667.180284	324413.324883	37.107213
1668.359375	324999.145251	37.112231
1670.448064	325579.021176	37.117248
1672.222653	326174.659991	37.122266
1673.928646	326756.568576	37.127284
1675.612189	327328.192631	37.132301
1677.245590	327928.001732	37.137319
1679.410713	328501.693430	37.142336
1680.541916	329106.981558	37.147354
1682.498105	329695.675680	37.152372
1684.471565	330281.593774	37.157389
1686.160910	330889.488139	37.162407
1688.203147	331475.357526	37.167424
1689.259786	332070.624616	37.172442
1690.859138	332671.635039	37.177460
1692.755037	333262.613098	37.182477
1693.928177	333864.823558	37.187495
1695.719598	334482.918957	37.192512
1697.628319	335107.588491	37.197530
1699.023925	335715.631688	37.202548
1700.974896	336327.257374	37.207565
1702.197655	336953.948185	37.212583
1704.169663	337567.866343	37.217600
1705.977054	338193.100738	37.222618
1707.388541	338811.970782	37.227636
1709.456596	339440.345739	37.232653
1710.917533	340081.733563	37.237671
1712.857089	340691.736658	37.242688
1715.063025	341315.268488	37.247706
1716.703265	341948.201454	37.252724
1718.945361	342557.446819	37.257741
1720.062678	343183.114894	37.262759
1722.179234	343818.356844	37.267776
1723.663846	344444.405189	37.272794
1725.370962	345065.941694	37.277812
1727.169746	345687.886564	37.282829
1728.775731	346317.215541	37.287847
1730.448000	346942.794384	37.292864
1731.752106	347570.532221	37.297882
1733.758911	348201.115149	37.302900
1735.873459	348841.163588	37.307917
1737.257526	349469.319497	37.312935
1739.165767	350102.988993	37.317952
1741.091036	350743.752755	37.322970
1742.565066	351376.283366	37.327988
1744.531536	352015.321972	37.333005
1746.361990	352655.008301	37.338023
1748.090464	353276.735538	37.343040
1749.928587	353898.715053	37.348058
1751.583797	354519.548609	37.353076
1753.586785	355120.040815	37.358093
1755.055862	355725.205672	37.363111
1756.890013	356333.448259	37.368128
1758.718392	356932.700535	37.373146
1760.102936	357542.649335	37.378164
1762.577132	358144.315300	37.383181
1763.556471	358758.043235	37.388199
1765.378531	359377.864868	37.393216
1767.299738	360003.471188	37.398234
1768.510873	360626.901608	37.403252
1770.503916	361251.741201	37.408269
1771.865237	361889.995414	37.413287
1773.496580	362512.820088	37.418304
1775.153432	363162.498436	37.423322
1776.531271	363821.649943	37.428340
1778.331768	364462.505185	37.433357
1779.952082	365134.025969	37.438375
1781.997882	365797.423041	37.443392
1783.944981	366457.653977	37.448410
1785.096401	367120.110413	37.453428
1787.199261	367794.752498	37.458445
1789.037960	368479.167209	37.463463
1790.213284	369144.476326	37.468480
1792.115394	369838.038671	37.473498
1793.688437	370530.830708	37.478516
1795.707819	371215.977307	37.483533
1797.939763	371906.554922	37.488551
1799.342652	372600.832659	37.493568
1801.524680	373296.414375	37.498586
1803.139504	374012.265560	37.503604
1805.187170	374709.592259	37.508621
1806.768417	375412.764917	37.513639
1808.463252	376126.252573	37.518656
1810.392795	376837.683537	37.523674
1812.170290	377552.751755	37.528692
1814.195426	378252.751124	37.533709
1815.993718	378971.920446	37.538727
1818.277736	379685.009828	37.543744
1820.050518	380390.459613	37.548762
1821.764733	381108.710348	37.553780
1824.175521	381823.864072	37.558797
1825.838936	382534.485501	37.563815
1827.741616	383228.925532	37.568832
1829.685192	383951.945981	37.573850
1831.372112	384667.082014	37.578868
1833.160170	385364.969752	37.583885
1834.561492	386104.918669	37.588903
1836.534573	386823.053512	37.593920
1838.533091	387529.353541	37.598938
1840.180237	388264.293864	37.603956
1842.387668	388979.679745	37.608973
1844.184646	389706.373294	37.613991
1845.808590	390433.636367	37.619008
1847.637472	391163.738717	37.624026
1849.674690	391889.530845	37.629044
1851.860839	392609.628547	37.634061
1853.285180	393338.859201	37.639079
1855.220479	394066.746184	37.644096
1857.404363	394796.881406	37.649114
1859.030853	395528.637148	37.654132
1861.011405	396251.470926	37.659149
1862.901806	396984.364346	37.664167
1864.827328	397719.515018	37.669184
1866.753765	398429.404397	37.674202
1868.805531	399142.880184	37.679220
1870.893673	399871.766576	37.684237
1872.949603	400576.818190	37.689255
1874.777633	401261.566122	37.694272
1876.898458	401946.452277	37.699290
1878.785149	402645.728903	37.704308
1881.111760	403321.374995	37.709325
1883.157116	403990.336504	37.714343
1884.551790	404673.173895	37.719360
1886.617304	405356.542914	37.724378
1888.052464	406034.425009	37.729396
1890.423146	406720.978973	37.734413
1892.033866	407410.555030	37.739431
1893.649619	408100.569132	37.744448
1895.240760	408787.884503	37.749466
1896.649141	409500.091232	37.754484
1898.865976	410214.502077	37.759501
1900.788544	410926.434695	37.764519
1902.305865	411631.170333	37.769536
1904.223159	412358.240163	37.774554
1905.741504	413081.911033	37.779572
1907.712059	413822.788316	37.784589
1909.077962	414560.173153	37.789607
1911.180004	415304.558738	37.794624
1913.129514	416043.806753	37.799642
1915.332542	416793.148375	37.804660
1917.203442	417533.126954	37.809677
1919.385280	418287.165031	37.814695
1920.930233	419029.180585	37.819712
1923.120239	419782.565629	37.824730
1924.836678	420539.247984	37.829748
1926.824125	421299.965428	37.834765
1928.996738	422068.808529	37.839783
1930.927613	422832.451764	37.844800
1933.062481	423603.305104	37.849818
1934.574752	424362.109019	37.854836
1936.615074	425113.991756	37.859853
1938.893552	425894.143591	37.864871
1940.509721	426682.025786	37.869888
1942.790051	427445.519577	37.874906
1944.258365	428222.287640	37.879924
1946.706272	428999.578041	37.884941
1948.560464	429775.068028	37.889959
1950.226029	430554.512962	37.894976
1952.765009	431345.837229	37.899994
1954.181146	432131.954224	37.905012
1956.257234	432911.203520	37.910029
1958.454110	433692.685013	37.915047
1960.414136	434501.614782	37.920064
1962.655514	435266.079110	37.925082
1964.331463	436058.196806	37.930100
1966.615458	436855.805160	37.935117
1968.753939	437635.948826	37.940135
1970.454204	438429.144950	37.945152
1972.855446	439222.703946	37.950170
1974.573240	440013.007889	37.955188
1976.891444	440787.092880	37.960205
1978.667864	441581.431145	37.965223
1980.820820	442363.383065	37.970240
1982.591003	443142.233528	37.975258
1984.873468	443932.103637	37.980276
1986.836722	444723.971391	37.985293
1989.118881	445507.157086	37.990311
1990.961903	446281.128847	37.995328
1992.915747	447064.312900	38.000346
1994.924593	447857.071453	38.005364
1997.172132	448640.048949	38.010381
1999.090835	449415.262150	38.015399
2001.034118	450199.952871	38.020416
2003.126043	450987.928594	38.025434
2004.965589	451773.236043	38.030452
2006.893048	452529.721349	38.035469
2008.821835	453291.186283	38.040487
2010.479856	454057.068182	38.045504
2012.721196	454810.789732	38.050522
2014.464698	455578.472883	38.055540
2016.210423	456347.189201	38.060557
2018.368572	457120.916106	38.065575
2020.137610	457901.807674	38.070592
2022.295035	458681.341387	38.075610
2024.129038	459455.235905	38.080628
2025.745663	460240.158592	38.085645
2028.350899	461033.431884	38.090663
2029.670405	461828.200440	38.095680
2031.497421	462629.981778	38.100698
2033.292892	463447.052995	38.105716
2035.411322	464252.512416	38.110733
2037.250101	465066.173781	38.115751
2039.320874	465904.125715	38.120768
2041.560750	466722.504851	38.125786
2043.441140	467555.009759	38.130804
2045.637436	468394.300210	38.135821
2047.547874	469223.544990	38.140839
2049.502544	470073.061399	38.145856
2051.397476	470906.026540	38.150874
2053.451499	471765.052799	38.155892
2055.593768	472616.851132	38.160909
2057.798499	473474.562950	38.165927
2059.528080	474348.632977	38.170944
2061.483811	475201.861644	38.175962
2063.754669	476070.710575	38.180980
2066.019103	476943.460442	38.185997
2068.143426	477814.879253	38.191015
2070.604926	478686.959239	38.196032
2072.656705	479566.136798	38.201050
2074.828977	480446.767703	38.206068
2076.798881	481316.077020	38.211085
2079.025276	482187.777224	38.216103
2080.880818	483073.888848	38.221120
2082.988258	483947.140179	38.226138
2085.337492	484833.437670	38.231156
2087.185251	485720.834477	38.236173
2089.841068	486600.228362	38.241191
2092.005798	487482.184158	38.246208
2094.522168	488356.869541	38.251226
2096.433912	489258.971997	38.256244
2098.359353	490136.089770	38.261261
2101.071694	491015.860588	38.266279
2102.974457	491899.657544	38.271296
2105.325230	492766.680457	38.276314
2107.366215	493652.232917	38.281332
2109.309883	494533.769269	38.286349
2111.497014	495419.257360	38.291367
2113.231590	496298.416349	38.296384
2115.395876	497180.083029	38.301402
2117.889464	498063.112911	38.306420
2119.606662	498954.448561	38.311437
2121.801166	499830.271264	38.316455
2123.969746	500727.492669	38.321472
2126.283515	501617.428531	38.326490
2128.236903	502500.163197	38.331508
2130.407376	503396.231990	38.336525
2132.606772	504293.155391	38.341543
2134.502828	505172.882210	38.346560
2136.468034	506062.334142	38.351578
2138.950008	506958.208209	38.356596
2140.752792	507865.289076	38.361613
2143.265467	508757.378047	38.366631
2145.200597	509643.563574	38.371648
2147.701798	510521.489944	38.376666
2149.585526	511379.052395	38.381684
2151.572506	512241.643483	38.386701
2153.802092	513100.216054	38.391719
2155.796097	513981.211849	38.396736
2157.927875	514845.906083	38.401754
2160.286096	515717.672507	38.406772
2162.112668	516591.494207	38.411789
2164.221537	517456.552731	38.416807
2165.927256	518342.844929	38.421824
2168.448447	519240.692894	38.426842
2170.355476	520141.562952	38.431860
2172.400115	521030.920798	38.436877
2174.640797	521929.464963	38.441895
2176.651105	522841.848300	38.446912
2178.658542	523756.293400	38.451930
2181.086642	524656.208034	38.456948
2182.932269	525597.316317	38.461965
2185.479686	526502.944318	38.466983
2187.173971	527433.738949	38.472000
2189.359686	528354.625208	38.477018
2191.753436	529305.785103	38.482036
2193.831660	530239.111495	38.487053
2196.404313	531175.016595	38.492071
2198.473749	532120.813363	38.497088
2200.778114	533058.254475	38.502106
2203.236419	533997.422632	38.507124
2205.430244	534950.869752	38.512141
2207.585441	535897.163934	38.517159
2209.746339	536850.894748	38.522176
2212.044145	537794.726480	38.527194
2214.486597	538751.959309	38.532212
2216.475737	539725.053964	38.537229
2218.596994	540662.839122	38.542247
2220.718596	541632.914089	38.547264
2223.085428	542604.391770	38.552282
2225.538137	543584.038949	38.557300
2227.304266	544549.747190	38.562317
2229.528040	545518.281381	38.567335
2232.000054	546510.698890	38.572352
2234.164073	547482.476844	38.577370
2236.596599	548465.960570	38.582388
2238.540640	549450.963673	38.587405
2240.905865	550435.374613	38.592423
2243.181179	551431.444799	38.597440
2245.438293	552421.915518	38.602458
2247.961003	553408.399864	38.607476
2249.889268	554402.802737	38.612493
2252.994436	555388.444232	38.617511
2254.874844	556372.657805	38.622528
2256.975653	557364.502637	38.627546
2259.434021	558362.697849	38.632564
2261.474822	559365.912344	38.637581
2264.107047	560355.488296	38.642599
2266.224457	561365.071391	38.647616
2268.128571	562359.742526	38.652634
2270.854739	563361.235864	38.657652
2273.313548	564355.966277	38.662669
2275.606405	565351.100611	38.667687
2277.596600	566349.724590	38.672704
2279.808236	567351.549868	38.677722
2282.109091	568347.709318	38.682740
2284.315415	569360.628059	38.687757
2286.835433	570361.918220	38.692775
2289.020571	571367.753945	38.697792
2291.347062	572389.751607	38.702810
2293.417699	573392.334529	38.707828
2295.437475	574391.935718	38.712845
2298.237648	575375.620982	38.717863
2300.109406	576357.525915	38.722880
2302.329440	577344.214342	38.727898
2304.848415	578311.257863	38.732916
2306.363536	579298.661151	38.737933
2308.915015	580288.123030	38.742951
2311.505879	581279.004476	38.747968
2313.046637	582273.189912	38.752986
2315.689324	583272.279534	38.758004
2317.239825	584284.005737	38.763021
2319.689980	585292.040020	38.768039
2321.843448	586314.130054	38.773056
2323.916580	587349.885389	38.778074
2326.349617	588379.376677	38.783092
2328.407013	589426.638247	38.788109
2330.965693	590479.239959	38.793127
2333.432239	591530.862462	38.798144
2335.309082	592580.435058	38.803162
2337.702186	593638.098694	38.808180
2339.751323	594713.412869	38.813197
2342.497166	595773.383589	38.818215
2344.991273	596844.973586	38.823232
2347.157538	597921.579550	38.828250
2349.810891	599004.417817	38.833268
2351.506415	600092.472399	38.838285
2354.339597	601170.923012	38.843303
2356.758331	602266.767899	38.848320
2359.040531	603370.592837	38.853338
2361.641477	604461.042305	38.858356
2363.688761	605560.240217	38.863373
2366.389024	606660.326236	38.868391
2368.601335	607770.446937	38.873408
2370.773806	608886.921835	38.878426
2373.438383	609983.689605	38.883444
2375.516990	611110.569365	38.888461
2377.854604	612229.138577	38.893479
2380.367319	613358.223017	38.898496
2382.764086	614490.463956	38.903514
2384.755871	615618.655355	38.908532
2387.373021	616764.132904	38.913549
2389.521427	617908.569071	38.918567
2391.453341	619048.972164	38.923584
2394.452201	620201.079948	38.928602
2397.444397	621357.566753	38.933620
2399.618506	622503.519124	38.938637
2402.039590	623656.707052	38.943655
2404.373883	624793.944832	38.948672
2406.481179	625955.185359	38.953690
2408.975886	627115.437400	38.958708
2411.571097	628288.036940	38.963725
2413.870200	629441.325013	38.968743
2416.205414	630608.967027	38.973760
2418.479569	631789.675343	38.978778
2421.001713	632957.028001	38.983796
2423.090123	634128.916607	38.988813
2425.457311	635308.666566	38.993831
2427.882005	636498.707344	38.998848
2430.156280	637683.496222	39.003866
2432.637346	638865.221488	39.008884
2434.858141	640062.673991	39.013901
2437.222179	641275.930969	39.018919
2439.595563	642480.612049	39.023936
2442.185043	643671.397898	39.028954
2444.696505	644876.323321	39.033972
2446.983835	646084.634396	39.038989
2449.227254	647293.457304	39.044007
2451.832264	648497.339538	39.049024
2454.639966	649699.249972	39.054042
2457.313415	650863.452721	39.059060
2459.479385	652041.709591	39.064077
2462.007002	653203.471085	39.069095
2464.600246	654372.810159	39.074112
2466.815921	655557.469892	39.079130
2469.632089	656726.046148	39.084148
2471.701198	657903.025641	39.089165
2474.068240	659084.098615	39.094183
2476.339970	660262.704280	39.099200
2478.874929	661461.391232	39.104218
2481.437495	662649.768979	39.109236
2483.653380	663859.913298	39.114253
2485.905638	665056.659498	39.119271
2488.569920	666264.387726	39.124288
2490.689948	667486.634944	39.129306
2493.168242	668703.293258	39.134324
2495.660358	669935.068093	39.139341
2497.683055	671159.647256	39.144359
2500.424641	672396.036405	39.149376
2502.455227	673653.368123	39.154394
2504.780022	674909.837131	39.159412
2507.709006	676181.650198	39.164429
2509.750915	677453.486345	39.169447
2512.602264	678709.259013	39.174464
2514.833521	679994.336182	39.179482
2517.613528	681264.883114	39.184500
2520.411666	682558.951913	39.189517
2522.541637	683846.689451	39.194535
2525.068805	685134.478744	39.199552
2527.685120	686436.077110	39.204570
2530.180263	687743.071017	39.209588
2532.794968	689051.346541	39.214605
2535.699114	690361.569441	39.219623
2538.146254	691677.385308	39.224640
2540.175086	692982.754890	39.229658
2542.644109	694313.068905	39.234676
2545.467443	695644.813094	39.239693
2547.892861	696962.434698	39.244711
2550.448381	698310.292333	39.249728
2552.654975	699653.737073	39.254746
2555.301223	700999.829777	39.259764
2557.756485	702348.771564	39.264781
2560.175378	703701.674960	39.269799
2563.039826	705043.143906	39.274816
2565.519672	706409.096537	39.279834
2568.192647	707772.076847	39.284852
2570.743821	709138.279901	39.289869
2573.236858	710497.490001	39.294887
2575.861880	711871.318962	39.299904
2578.056570	713254.058644	39.304922
2580.983720	714624.621305	39.309940
2583.688613	715993.167703	39.314957
2586.410967	717385.788536	39.319975
2589.343946	718761.469492	39.324992
2591.752912	720141.859643	39.330010
2594.285521	721514.829355	39.335028
2597.339385	722895.449486	39.340045
2599.712968	724280.105949	39.345063
2602.217098	725655.808051	39.350080
2604.513154	727035.665114	39.355098
2607.742275	728420.375776	39.360116
2610.519935	729797.415939	39.365133
2613.161436	731182.843161	39.370151
2615.668901	732562.079666	39.375168
2618.470688	733937.576053	39.380186
2621.346478	735298.851535	39.385204
2623.994757	736681.708065	39.390221
2626.597609	738038.121767	39.395239
2629.348343	739381.745027	39.400256
2631.808038	740705.796518	39.405274
2634.563545	742042.061939	39.410292
2637.117887	743373.251701	39.415309
2639.694547	744714.029021	39.420327
2641.921054	746031.162368	39.425344
2644.707009	747374.558894	39.430362
2646.684114	748714.161090	39.435380
2649.885717	750060.626576	39.440397
2652.233110	751414.737058	39.445415
2655.039947	752752.522188	39.450432
2657.713439	754116.109133	39.455450
2660.074065	755487.584357	39.460468
2662.822044	756853.038606	39.465485
2665.156239	758234.073652	39.470503
2668.192607	759590.916916	39.475520
2670.650002	760970.746973	39.480538
2673.263622	762339.966332	39.485556
2675.763981	763748.170152	39.490573
2677.972532	765153.060107	39.495591
2681.206252	766546.304942	39.500608
2684.089803	767946.478683	39.505626
2686.736852	769354.295322	39.510644
2689.644617	770770.896582	39.515661
2691.980440	772197.101769	39.520679
2694.835306	773608.549638	39.525696
2697.565458	775042.739301	39.530714
2700.056380	776462.051712	39.535732
2702.790068	777898.875323	39.540749
2705.263525	779352.790752	39.545767
2708.008513	780786.490477	39.550784
2710.564968	782242.072380	39.555802
2713.167540	783709.669967	39.560820
2715.820851	785157.778685	39.565837
2718.405791	786621.940040	39.570855
2721.013434	788088.642640	39.575872
2723.287933	789577.847960	39.580890
2725.866334	791069.730725	39.585908
2729.205693	792563.722715	39.590925
2731.664643	794061.512834	39.595943
2734.729239	795567.261521	39.600960
2737.226516	797068.373029	39.605978
2739.930009	798577.550760	39.610996
2742.889573	800086.310908	39.616013
2745.836326	801605.024116	39.621031
2748.580044	803106.017669	39.626048
2751.158905	804621.682687	39.631066
2753.894726	806138.259947	39.636084
2756.646997	807662.812583	39.641101
2759.401862	809189.713981	39.646119
2762.244517	810708.389391	39.651136
2765.078532	812232.639902	39.656154
2767.107695	813769.236363	39.661172
2770.453934	815300.137234	39.666189
2773.582327	816843.520427	39.671207
2776.311372	818374.652413	39.676224
2779.096080	819900.299194	39.681242
2782.071132	821443.231355	39.686260
2785.070733	822977.018779	39.691277
2787.960098	824520.614908	39.696295
2791.051174	826042.700415	39.701312
2793.625467	827565.250110	39.706330
2796.267928	829111.758499	39.711348
2799.387337	830650.707226	39.716365
2801.637110	832179.886153	39.721383
2804.522522	833704.654626	39.726400
2807.558173	835246.960090	39.731418
2810.289493	836764.603427	39.736436
2812.981278	838269.823500	39.741453
2815.908913	839761.609187	39.746471
2818.688289	841255.649564	39.751488
2821.230271	842752.832125	39.756506
2823.586210	844244.197130	39.761524
2826.333096	845748.953971	39.766541
2828.611198	847258.873160	39.771559
2831.323184	848763.110161	39.776576
2834.241863	850310.968656	39.781594
2836.200787	851847.042073	39.786612
2839.256096	853391.782412	39.791629
2842.379516	854932.049356	39.796647
2845.402092	856468.163970	39.801664
2848.180393	858029.653525	39.806682
2850.855437	859600.368790	39.811700
2853.591970	861154.861307	39.816717
2856.424330	862751.900773	39.821735
2859.123767	864328.378939	39.826752
2861.766596	865919.092142	39.831770
2864.147498	867521.251632	39.836788
2866.967815	869123.978892	39.841805
2869.753602	870742.747956	39.846823
2872.370928	872369.433841	39.851840
2875.590898	874014.741885	39.856858
2877.927797	875646.871415	39.861876
2881.391372	877292.973670	39.866893
2884.204707	878950.039922	39.871911
2887.185908	880594.334258	39.876928
2890.569728	882242.934903	39.881946
2893.249229	883897.275065	39.886964
2896.702486	885547.058357	39.891981
2899.804078	887216.325667	39.896999
2902.755319	888876.930994	39.902016
2905.008087	890534.954451	39.907034
2907.958335	892204.929407	39.912052
2911.536154	893883.961317	39.917069
2913.867708	895555.859239	39.922087
2916.761026	897235.272523	39.927104
2919.776128	898914.747885	39.932122
2922.538892	900601.089359	39.937140
2925.249098	902293.389243	39.942157
2928.337611	903988.295529	39.947175
2931.108034	905688.902731	39.952192
2934.457423	907393.035183	39.957210
2936.705033	909099.329205	39.962228
2939.784550	910818.618241	39.967245
2942.892146	912553.039517	39.972263
2945.686602	914263.996701	39.977280
2948.975932	915984.716616	39.982298
2951.621292	917711.149474	39.987316
2954.451379	919446.512105	39.992333
2957.695023	921164.359259	39.997351
2960.398251	922885.397868	40.002368
2963.391395	924637.113357	40.007386
2966.171910	926379.471950	40.012404
2969.379860	928110.649642	40.017421
2972.386388	929855.484031	40.022439
2975.042662	931603.062695	40.027456
2978.028163	933352.694287	40.032474
2980.725645	935108.305867	40.037492
2984.065454	936850.116031	40.042509
2987.020904	938620.307111	40.047527
2989.722590	940379.995693	40.052544
2992.689911	942137.327197	40.057562
2995.403223	943906.628626	40.062580
2998.412017	945660.564413	40.067597
3001.792986	947444.599809	40.072615
3004.568939	949204.247623	40.077632
3007.429924	950935.026408	40.082650
3009.944869	952679.589928	40.087668
3012.607811	954413.708608	40.092685
3015.594909	956199.978402	40.097703
3018.336796	957986.782207	40.102720
3021.308662	959775.243919	40.107738
3023.907869	961592.732478	40.112756
3026.839503	963400.114457	40.117773
3029.814252	965219.718961	40.122791
3032.318596	967057.672988	40.127808
3035.444966	968890.153296	40.132826
3038.299430	970749.907711	40.137844
3041.268550	972609.138082	40.142861
3043.602707	974486.790858	40.147879
3046.600787	976369.081227	40.152896
3049.442904	978253.897154	40.157914
3052.054151	980166.872550	40.162932
3055.289814	982083.585026	40.167949
3057.936252	984016.692839	40.172967
3060.570462	985948.271518	40.177984
3064.364478	987873.847482	40.183002
3067.367090	989845.882704	40.188020
3070.703327	991800.649595	40.193037
3073.495707	993765.136906	40.198055
3076.135348	995736.645872	40.203072
3079.388000	997713.390931	40.208090
3081.879649	999715.108754	40.213108
3084.889915	1001714.771744	40.218125
3088.519042	1003729.441735	40.223143
3091.560506	1005749.503991	40.228160
3094.799960	1007764.253841	40.233178
3097.591788	1009791.830456	40.238196
3100.450005	1011814.306674	40.243213
3103.817156	1013842.365074	40.248231
3106.933787	1015898.005041	40.253248
3110.465850	1017934.629149	40.258266
3113.635991	1019960.608843	40.263284
3116.730610	1022008.403750	40.268301
3119.995862	1024053.005259	40.273319
3122.711962	1026111.157166	40.278336
3126.181935	1028155.771899	40.283354
3128.949687	1030235.872317	40.288372
3132.595442	1032296.711110	40.293389
3135.580417	1034355.932153	40.298407
3137.993049	1036436.384019	40.303424
3141.337513	1038516.676288	40.308442
3144.244933	1040611.781506	40.313460
3146.939203	1042700.832124	40.318477
3150.193028	1044790.641693	40.323495
3153.190285	1046911.864467	40.328512
3156.278897	1049015.609206	40.333530
3159.570782	1051137.762582	40.338548
3162.483957	1053257.240158	40.343565
3165.754897	1055379.210102	40.348583
3168.760662	1057512.708132	40.353600
3172.277785	1059624.738837	40.358618
3175.376004	1061768.580618	40.363636
3178.717203	1063889.277735	40.368653
3182.217919	1066015.942476	40.373671
3185.313498	1068157.100062	40.378688
3188.896750	1070266.852836	40.383706
3191.945691	1072390.735988	40.388724
3195.333071	1074506.458171	40.393741
3198.913980	1076637.226473	40.398759
3202.210642	1078759.169133	40.403776
3205.663352	1080857.199493	40.408794
3209.027919	1082966.488974	40.413812
3212.186744	1085059.027275	40.418829
3215.214827	1087119.527507	40.423847
3218.215237	1089184.314761	40.428864
3221.561519	1091231.068322	40.433882
3224.122597	1093286.534902	40.438900
3227.480917	1095346.625601	40.443917
3230.737355	1097417.587536	40.448935
3233.480642	1099488.603647	40.453952
3236.721387	1101560.840955	40.458970
3239.588453	1103645.589124	40.463988
3242.148726	1105735.296716	40.469005
3245.374095	1107827.035575	40.474023
3248.446749	1109949.299591	40.479040
3251.638422	1112075.462918	40.484058
3254.494241	1114209.874199	40.489076
3257.361927	1116352.179978	40.494093
3260.406396	1118504.052851	40.499111
3262.986343	1120684.108043	40.504128
3266.669060	1122855.876705	40.509146
3269.122918	1125050.312241	40.514164
3272.554976	1127250.609640	40.519181
3276.026812	1129470.001264	40.524199
3278.950270	1131703.155689	40.529216
3281.961359	1133928.820165	40.534234
3285.343037	1136177.452962	40.539252
3288.808862	1138428.148449	40.544269
3291.769017	1140674.754087	40.549287
3295.300248	1142942.068111	40.554304
3298.393625	1145214.627917	40.559322
3301.732684	1147493.824869	40.564340
3304.707435	1149776.631850	40.569357
3308.191657	1152072.530270	40.574375
3311.134165	1154375.822631	40.579392
3314.333029	1156682.969949	40.584410
3317.352885	1159008.559676	40.589428
3320.877872	1161328.793853	40.594445
3324.469573	1163659.296044	40.599463
3327.513815	1165993.748080	40.604480
3331.043917	1168324.065690	40.609498
3334.530490	1170664.453604	40.614516
3337.820835	1173012.194326	40.619533
3341.390091	1175353.190970	40.624551
3344.831011	1177705.277278	40.629568
3348.383227	1180043.132016	40.634586
3352.030223	1182379.730842	40.639604
3355.291356	1184728.947020	40.644621
3358.956987	1187073.560929	40.649639
3362.237705	1189430.957461	40.654656
3365.709938	1191781.062438	40.659674
3369.211984	1194124.659991	40.664692
3372.600698	1196473.203000	40.669709
3375.943289	1198807.674836	40.674727
3379.550061	1201170.882781	40.679744
3382.994101	1203511.152554	40.684762
3386.462754	1205858.014308	40.689780
3389.731062	1208198.790444	40.694797
3393.112514	1210529.421133	40.699815
3396.337507	1212890.186137	40.704832
3399.864709	1215237.123990	40.709850
3403.357656	1217587.556597	40.714868
3406.147947	1219950.254661	40.719885
3409.705182	1222298.874685	40.724903
3413.235470	1224670.250182	40.729920
3416.481997	1227033.026600	40.734938
3419.900450	1229397.092562	40.739956
3423.312420	1231771.492742	40.744973
3426.653757	1234128.805361	40.749991
3429.788690	1236496.942556	40.755008
3433.484382	1238847.293252	40.760013
3436.469352	1241153.416913	40.765018
3439.857874	1243394.804872	40.770023
3443.420383	1245563.770909	40.775028
3446.864890	1247669.004276	40.780032
3449.958655	1249691.859274	40.785037
3453.370243	1251651.358463	40.790042
3456.178497	1253527.121939	40.795047
3459.063419	1255299.925221	40.800052
3461.875342	1257014.328951	40.805056
3464.243347	1258637.909120	40.810061
3466.805486	1260194.470255	40.815066
3469.308130	1261685.876874	40.820071
3471.978005	1263096.401428	40.825076
3473.813333	1264438.964996	40.830080
3476.033592	1265705.458921	40.835085
3478.630917	1266909.456867	40.840090
3480.172791	1268052.628031	40.845095
3482.158234	1269110.063407	40.850100
3484.296639	1270127.193419	40.855104
3485.652754	1271080.149902	40.860109
3487.583751	1271984.651332	40.865114
3489.289240	1272818.943988	40.870119
3490.572117	1273602.231022	40.875124
3492.325481	1274344.094362	40.880128
3493.447581	1275025.511845	40.885133
3494.888487	1275660.397162	40.890138
3495.950842	1276270.410168	40.895143
3497.629753	1276809.113541	40.900148
3498.301137	1277341.088636	40.905152
3499.459910	1277810.951533	40.910157
3500.546253	1278240.053618	40.915162
3501.531102	1278663.594346	40.920167
3502.907780	1279018.980370	40.925172
3503.513062	1279348.152857	40.930176
3504.320872	1279629.628914	40.935181
3505.079120	1279908.327382	40.940186
3505.952163	1280157.080148	40.945191
3506.826963	1280374.710269	40.950196
3507.387960	1280558.966060	40.955200
3507.894928	1280717.100811	40.960205
3508.727746	1280849.792918	40.965210
3509.407607	1280977.983795	40.970215
3510.413165	1281077.042938	40.975220
3510.390383	1281146.456688	40.980224
3511.337602	1281199.095962	40.985229
3511.856011	1281241.744814	40.990234
3511.778765	1281246.095598	40.995239
3512.995411	1281245.249211	41.000244
3513.090589	1281227.235463	41.005248
3513.603896	1281188.939352	41.010253
3514.139530	1281130.887089	41.015258
3514.126437	1281066.832631	41.020263
3514.695588	1280987.451523	41.025268
3514.860112	1280901.674473	41.030272
3515.251430	1280792.966650	41.035277
3516.033435	1280672.838145	41.040282
3516.081995	1280539.257786	41.045287
3516.090012	1280391.187225	41.050292
3516.360255	1280238.822467	41.055296
3516.918617	1280089.729065	41.060301
3516.671312	1279921.745405	41.065306
3517.040986	1279743.406241	41.070311
3517.339890	1279559.070880	41.075316
3517.977859	1279370.517819	41.080320
3518.120891	1279157.939180	41.085325
3517.905846	1278951.874222	41.090330
3518.425267	1278743.648126	41.095335
3518.893447	1278502.453132	41.100340
3519.093935	1278271.541706	41.105344
3518.659575	1278023.730160	41.110349
3519.132832	1277789.241663	41.115354
3519.025431	1277530.360367	41.120359
3519.520759	1277271.920484	41.125364
3519.490970	1277015.216359	41.130368
3519.719910	1276747.739991	41.135373
3519.882332	1276476.657016	41.140378
3519.621829	1276202.025533	41.145383
3520.239387	1275922.337132	41.150388
3520.226227	1275635.529380	41.155392
3520.144399	1275350.010021	41.160397
3520.563372	1275048.219328	41.165402
3520.255182	1274757.158206	41.170407
3520.370766	1274452.978281	41.175412
3520.362933	1274157.118733	41.180416
3520.423831	1273848.751317	41.185421
3520.402980	1273529.747328	41.190426
3520.498813	1273226.697063	41.195431
3520.770543	1272910.748246	41.200436
3520.836530	1272599.251223	41.205440
3520.624739	1272273.725616	41.210445
3520.824205	1271965.495530	41.215450
3520.659878	1271641.030198	41.220455
3520.850213	1271325.363618	41.225460
3520.883594	1271006.003223	41.230464
3520.881913	1270674.973629	41.235469
3521.075076	1270347.497411	41.240474
3520.715462	1270018.517980	41.245479
3521.352774	1269676.493120	41.250484
3520.947950	1269342.388025	41.255488
3520.846461	1269011.726478	41.260493
3521.169538	1268678.844734	41.265498
3521.093516	1268336.104738	41.270503
3520.830860	1267998.646901	41.275508
3521.047310	1267665.992457	41.280512
3521.154466	1267313.063567	41.285517
3521.197733	1266973.819674	41.290522
3520.958583	1266639.690514	41.295527
3521.135133	1266292.879962	41.300532
3520.932388	1265938.608409	41.305536
3520.991556	1265610.286264	41.310541
3521.299139	1265258.011739	41.315546
3521.012963	1264916.274163	41.320551
3521.046068	1264567.885275	41.325556
3520.782552	1264212.759891	41.330560
3521.000886	1263863.179767	41.335565
3521.086945	1263512.114814	41.340570
3520.501150	1263171.788800	41.345575
3520.830591	1262823.043686	41.350580
3520.795964	1262473.222332	41.355584
3520.531061	1262126.749895	41.360589
3520.976434	1261775.781311	41.365594
3520.717799	1261440.101422	41.370599
3520.782844	1261079.972392	41.375604
3520.555939	1260735.157720	41.380608
3520.504255	1260390.568396	41.385613
3520.914700	1260041.800644	41.390618
3520.391616	1259706.603702	41.395623
3520.653250	1259348.356601	41.400628
3520.673228	1259000.229270	41.405632
3520.476438	1258659.530876	41.410637
3520.733336	1258306.494737	41.415642
3520.369202	1257957.894315	41.420647
3520.749284	1257588.373502	41.425652
3520.365256	1257252.246817	41.430656
3520.404631	1256906.474366	41.435661
3520.789245	1256550.046697	41.440666
3520.593610	1256195.822754	41.445671
3520.794974	1255839.560115	41.450676
3520.860072	1255497.025653	41.455680
3520.736486	1255132.787257	41.460685
3520.626222	1254782.067635	41.465690
3520.507738	1254437.913386	41.470695
3520.370417	1254074.528126	41.475700
3520.280494	1253721.132226	41.480704
3520.183745	1253362.700348	41.485709
3520.249478	1253012.663013	41.490714
3520.119682	1252666.346609	41.495719
3520.315931	1252302.127868	41.500724
3520.215444	1251961.142396	41.505728
3520.080555	1251616.982477	41.510733
3520.218147	1251254.925623	41.515738
3520.223262	1250913.294276	41.520743
3520.199419	1250557.621144	41.525748
3520.033312	1250214.298683	41.530752
3520.117380	1249853.170987	41.535757
3520.262613	1249504.732997	41.540762
3520.055274	1249154.842531	41.545767
3519.849377	1248799.167491	41.550772
3520.164707	1248451.836057	41.555776
3520.096176	1248102.685499	41.560781
3520.061367	1247748.580255	41.565786
3519.693406	1247395.341239	41.570791
3519.742386	1247029.462517	41.575796
3519.954935	1246692.249036	41.580800
3519.736796	1246347.276265	41.585805
3520.169414	1245973.078016	41.590810
3519.780671	1245633.661574	41.595815
3520.164646	1245287.029451	41.600820
3519.807136	1244932.685762	41.605824
3519.611130	1244584.613125	41.610829
3520.151434	1244230.165028	41.615834
3519.598787	1243875.035005	41.620839
3519.983763	1243518.702479	41.625844
3519.886217	1243179.165278	41.630848
3519.398524	1242828.042862	41.635853
3519.385563	1242473.562083	41.640858
3519.454547	1242131.043120	41.645863
3519.681396	1241788.195752	41.650868
3519.542991	1241440.547210	41.655872
3519.509318	1241081.785098	41.660877
3519.782359	1240724.900990	41.665882
3519.272436	1240370.167814	41.670887
3519.619585	1240021.410747	41.675892
3519.481231	1239673.360995	41.680896
3519.361390	1239330.310316	41.685901
3519.712735	1238964.725530	41.690906
3519.454385	1238630.306806	41.695911
3519.391445	1238272.373418	41.700916
3519.253957	1237928.578568	41.705920
3519.428057	1237588.433338	41.710925
3519.334894	1237228.196195	41.715930
3519.314705	1236886.638907	41.720935
3518.966237	1236529.094433	41.725940
3519.020119	1236183.938489	41.730944
3518.830550	1235838.240188	41.735949
3519.060620	1235498.037976	41.740954
3519.068528	1235157.756282	41.745959
3519.109136	1234809.154996	41.750964
3518.897047	1234477.620792	41.755968
3519.159014	1234121.482265	41.760973
3518.967574	1233779.277079	41.765978
3518.776717	1233442.732955	41.770983
3518.852651	1233099.505853	41.775988
3519.143339	1232755.474497	41.780992
3518.762553	1232413.208008	41.785997
3518.946082	1232066.630917	41.791002
3518.763538	1231728.293501	41.796007
3518.571286	1231387.977359	41.801012
3518.618578	1231038.089421	41.806016
3518.466196	1230701.170032	41.811021
3518.708753	1230366.587478	41.816026
3518.369866	1230049.516022	41.821031
3518.656051	1229698.563677	41.826036
3518.466699	1229357.457745	41.831040
3518.341199	1229016.784659	41.836045
3518.722710	1228689.902901	41.841050
3518.265519	1228355.769116	41.846055
3518.178319	1228012.690224	41.851060
3518.060117	1227684.519919	41.856064
3518.183020	1227338.188855	41.861069
3518.313546	1227006.481671	41.866074
3518.250113	1226671.892115	41.871079
3518.077560	1226329.553176	41.876084
3517.974822	1225996.605249	41.881088
3517.470864	1225665.288139	41.886093
3518.155308	1225344.673861	41.891098
3517.868191	1225024.759390	41.896103
3518.011281	1224691.031940	41.901108
3517.752872	1224357.068619	41.906112
3517.855554	1224034.507021	41.911117
3517.696832	1223705.245717	41.916122
3517.686592	1223384.622112	41.921127
3517.667313	1223046.611660	41.926132
3517.553872	1222728.578210	41.931136
3517.122052	1222412.631842	41.936141
3517.454107	1222086.733595	41.941146
3517.066100	1221781.948157	41.946151
3517.349095	1221455.457133	41.951156
3517.376904	1221144.587006	41.956160
3517.378494	1220816.513314	41.961165
3517.329874	1220497.115161	41.966170
3516.870016	1220186.360212	41.971175
3517.112446	1219857.531014	41.976180
3517.151674	1219545.066306	41.981184
3516.751371	1219240.597799	41.986189
3516.816352	1218916.596288	41.991194
3516.796353	1218607.167716	41.996199
3516.607855	1218297.187309	42.001204
3516.990617	1217979.522884	42.006208
3516.496437	1217680.210851	42.011213
3516.908410	1217356.239896	42.016218
3516.517762	1217056.126295	42.021223
3516.688008	1216741.130804	42.026228
3516.501160	1216438.796953	42.031232
3516.675813	1216115.160210	42.036237
3516.744810	1215808.632672	42.041242
3516.447738	1215501.211843	42.046247
3516.450770	1215193.536017	42.051252
3516.491418	1214895.281640	42.056256
3515.938018	1214571.199203	42.061261
3516.683580	1214268.208992	42.066266
3516.179093	1213971.767643	42.071271
3516.475925	1213655.064029	42.076276
3516.372433	1213361.234115	42.081280
3516.307703	1213064.948345	42.086285
3516.218711	1212759.292812	42.091290
3516.141799	1212445.476282	42.096295
3516.483413	1212147.292507	42.101300
3516.173991	1211850.415125	42.106304
3515.712920	1211551.018594	42.111309
3516.356980	1211238.880987	42.116314
3515.907782	1210937.200294	42.121319
3515.891807	1210632.154282	42.126324
3516.028019	1210338.953506	42.131328
3515.840157	1210045.040369	42.136333
3516.199847	1209748.586025	42.141338
3515.940609	1209464.013340	42.146343
3515.951824	1209146.890115	42.151348
3515.881647	1208847.739051	42.156352
3515.491857	1208561.077621	42.161357
3515.599226	1208254.652165	42.166362
3515.494636	1207971.656683	42.171367
3515.733410	1207673.228981	42.176372
3515.515946	1207378.043616	42.181376
3515.497902	1207088.241230	42.186381
3515.601244	1206791.845215	42.191386
3515.520968	1206500.802075	42.196391
3515.389703	1206213.404537	42.201396
3515.425806	1205929.242495	42.206400
3515.361900	1205627.466303	42.211405
3515.445149	1205333.050547	42.216410
3515.026253	1205044.697829	42.221415
3514.956248	1204758.707947	42.226420
3515.446679	1204488.260596	42.231424
3515.229114	1204198.796266	42.236429
3515.348105	1203908.135440	42.241434
3514.835350	1203607.251554	42.246439
3514.897567	1203333.908158	42.251444
3515.057763	1203049.191135	42.256448
3514.779272	1202771.561707	42.261453
3514.918425	1202483.723092	42.266458
3514.543718	1202214.798482	42.271463
3514.976054	1201928.005540	42.276468
3514.676732	1201644.317696	42.281472
3514.648375	1201374.729438	42.286477
3514.803179	1201106.034658	42.291482
3514.446590	1200827.656531	42.296487
3514.354629	1200539.278093	42.301492
3514.710844	1200272.288547	42.306496
3514.510800	1200000.780599	42.311501
3514.661504	1199724.885562	42.316506
3514.410139	1199443.788628	42.321511
3514.431806	1199173.326178	42.326516
3514.617324	1198902.916341	42.331520
3514.180543	1198626.308568	42.336525
3514.553660	1198349.083388	42.341530
3514.294032	1198086.397929	42.346535
3514.215502	1197810.062600	42.351540
3514.361434	1197536.490786	42.356544
3514.067304	1197265.886224	42.361549
3514.044074	1196994.096573	42.366554
3514.200768	1196732.681259	42.371559
3513.873970	1196461.195048	42.376564
3513.700838	1196190.795636	42.381568
3513.734870	1195930.392354	42.386573
3514.108986	1195670.952559	42.391578
3513.781523	1195408.329353	42.396583
3513.820334	1195136.431450	42.401588
3514.003273	1194877.452636	42.406592
3513.457126	1194623.275737	42.411597
3513.944729	1194359.056367	42.416602
3513.574392	1194099.566180	42.421607
3513.666169	1193833.131295	42.426612
3513.527304	1193565.124053	42.431616
3513.353082	1193301.616920	42.436621
3513.364468	1193053.281729	42.441626
3513.467098	1192809.334273	42.446631
3513.498111	1192553.833122	42.451636
3513.851415	1192286.993508	42.456640
3513.427689	1192027.595730	42.461645
3513.435157	1191773.093193	42.466650
3513.363417	1191527.046967	42.471655
3513.538358	1191278.223609	42.476660
3513.698468	1191020.464265	42.481664
3513.478025	1190758.620168	42.486669
3513.426030	1190494.761636	42.491674
3513.388535	1190241.976509	42.496679
3513.247813	1189984.966850	42.501684
3513.594441	1189728.240088	42.506688
3513.200013	1189478.765916	42.511693
3513.549188	1189221.449621	42.516698
3513.196615	1188970.064089	42.521703
3513.160366	1188710.811855	42.526708
3513.239615	1188461.398570	42.531712
3513.070321	1188213.988476	42.536717
3512.905142	1187949.548551	42.541722
3513.036395	1187707.705843	42.546727
3512.753117	1187458.962077	42.551732
3512.990899	1187202.597977	42.556736
3512.801121	1186965.945226	42.561741
3512.896680	1186717.009359	42.566746
3512.800600	1186480.695148	42.571751
3512.905579	1186232.862988	42.576756
3512.884007	1185982.782506	42.581760
3512.848987	1185734.103040	42.586765
3513.065382	1185485.934604	42.591770
3512.825889	1185251.657297	42.596775
3512.626236	1184993.656694	42.601780
3512.823297	1184742.069203	42.606784
3512.522476	1184506.827533	42.611789
3512.846998	1184259.052919	42.616794
3512.578239	1184024.630842	42.621799
3512.607776	1183784.785670	42.626804
3512.533357	1183539.865199	42.631808
3512.085980	1183299.323314	42.636813
3512.471724	1183048.093026	42.641818
3512.435998	1182819.789162	42.646823
3512.005327	1182580.434614	42.651828
3512.296464	1182347.256197	42.656832
3512.218205	1182115.351755	42.661837
3512.128144	1181875.814463	42.666842
3511.915513	1181647.299858	42.671847
3511.826131	1181397.574006	42.676852
3512.263027	1181183.335007	42.681856
3511.833839	1180954.825567	42.686861
3512.023775	1180723.191308	42.691866
3512.243527	1180495.778729	42.696871
3511.848546	1180272.035430	42.701876
3512.195019	1180034.506879	42.706880
3511.820067	1179805.278755	42.711885
3511.975289	1179570.302962	42.716890
3512.146696	1179351.041050	42.721895
3512.029569	1179125.036545	42.726900
3512.017057	1178885.442644	42.731904
3511.726276	1178653.324316	42.736909
3512.232426	1178422.477240	42.741914
3511.894904	1178206.547544	42.746919
3511.603947	1177976.659701	42.751924
3511.777984	1177734.438620	42.756928
3511.573996	1177517.045223	42.761933
3511.906409	1177281.842557	42.766938
3511.898234	1177072.971634	42.771943
3511.923932	1176847.127183	42.776948
3511.700515	1176604.542049	42.781952
3511.511843	1176395.673649	42.786957
3512.109290	1176160.942024	42.791962
3511.967726	1175930.750643	42.796967
3511.884289	1175705.063056	42.801972
3511.794067	1175480.497733	42.806977
3511.788161	1175249.217168	42.811981
3511.952094	1175014.128231	42.816986
3511.863491	1174795.942315	42.821991
3511.674310	1174571.165541	42.826996
3511.926090	1174340.367728	42.832001
3511.615147	1174125.395347	42.837005
3511.545981	1173878.415588	42.842010
3511.567468	1173676.945338	42.847015
3511.368576	1173446.276405	42.852020
3511.630165	1173220.895700	42.857025
3511.345999	1173011.152902	42.862029
3511.251674	1172784.303299	42.867034
3511.457847	1172559.468878	42.872039
3511.329659	1172328.644520	42.877044
3511.552081	1172123.026118	42.882049
3511.019814	1171908.753139	42.887053
3511.664147	1171684.751930	42.892058
3511.056164	1171475.943801	42.897063
3510.983612	1171257.324057	42.902068
3510.693125	1171035.901287	42.907073
3511.353340	1170836.574167	42.912077
3511.238803	1170611.236915	42.917082
3511.018140	1170389.680879	42.922087
3510.877461	1170189.234558	42.927092
3511.093140	1169980.419564	42.932097
3510.827659	1169771.486763	42.937101
3510.950241	1169560.122891	42.942106
3510.818801	1169340.772063	42.947111
3511.162432	1169139.922610	42.952116
3511.190864	1168917.791259	42.957121
3510.797629	1168712.045441	42.962125
3510.367816	1168492.047518	42.967130
3510.531971	1168296.857463	42.972135
3510.684321	1168095.999367	42.977140
3510.750349	1167879.385967	42.982145
3510.657765	1167683.271448	42.987149
3510.896737	1167474.163619	42.992154
3510.526645	1167273.265546	42.997159
3510.203930	1167068.953658	43.002164
3510.758833	1166860.713223	43.007169
3510.421278	1166663.184751	43.012173
3510.586903	1166462.167264	43.017178
3510.374630	1166249.497259	43.022183
3510.323345	1166041.512858	43.027188
3510.461839	1165850.201086	43.032193
3510.289370	1165656.384128	43.037197
3510.578595	1165458.801340	43.042202
3510.213979	1165254.519848	43.047207
3510.308196	1165054.404304	43.052212
3510.187691	1164856.110767	43.057217
3510.129795	1164664.032461	43.062221
3510.174070	1164457.480372	43.067226
3510.104533	1164259.816949	43.072231
3509.684225	1164071.554477	43.077236
3510.028592	1163863.040486	43.082241
3510.143115	1163675.336863	43.087245
3510.196037	1163479.890811	43.092250
3510.386680	1163285.453899	43.097255
3509.703282	1163098.049918	43.102260
3510.224352	1162898.537390	43.107265
3509.859906	1162714.940518	43.112269
3509.821078	1162520.796433	43.117274
3509.554792	1162332.729482	43.122279
3509.296956	1162149.851095	43.127284
3510.033853	1161952.723634	43.132289
3509.913952	1161775.762286	43.137293
3509.860144	1161587.633591	43.142298
3509.873730	1161396.179573	43.147303
3509.893055	1161196.684886	43.152308
3509.959148	1160992.733103	43.157313
3509.844466	1160809.500834	43.162317
3510.091930	1160627.431188	43.167322
3510.205530	1160445.377268	43.172327
3509.876087	1160245.714798	43.177332
3510.034880	1160039.347664	43.182337
3509.905555	1159845.591985	43.187341
3510.026377	1159657.176192	43.192346
3509.934455	1159474.460703	43.197351
3509.732609	1159275.118394	43.202356
3509.695486	1159091.151540	43.207361
3509.682701	1158915.777729	43.212365
3509.626619	1158719.321153	43.217370
3509.696025	1158526.051287	43.222375
3509.408027	1158350.609361	43.227380
3509.643297	1158164.768643	43.232385
3509.416863	1157986.656802	43.237389
3509.568900	1157791.833324	43.242394
3509.401245	1157604.147838	43.247399
3509.416965	1157428.435930	43.252404
3509.149613	1157246.901181	43.257409
3509.339594	1157081.268360	43.262413
3509.466766	1156885.847906	43.267418
3509.415427	1156700.853808	43.272423
3509.369429	1156527.391929	43.277428
3509.540156	1156341.213551	43.282433
3509.341266	1156156.697542	43.287437
3509.307700	1155972.904599	43.292442
3509.017412	1155801.918517	43.297447
3509.105700	1155624.526114	43.302452
3509.251465	1155449.672630	43.307457
3509.176628	1155279.674741	43.312461
3509.326887	1155087.873381	43.317466
3508.922557	1154905.523363	43.322471
3508.774637	1154738.642342	43.327476
3508.872305	1154571.242467	43.332481
3508.945994	1154402.232586	43.337485
3509.011864	1154224.134248	43.342490
3508.935714	1154055.800311	43.347495
3508.823304	1153882.545965	43.352500
3508.994601	1153705.642958	43.357505
3508.541938	1153546.156014	43.362509
3508.854258	1153384.550733	43.367514
3508.976280	1153203.474645	43.372519
3508.713870	1153037.031716	43.377524
3508.811570	1152851.593637	43.382529
3508.471034	1152693.292855	43.387533
3508.506768	1152519.969238	43.392538
3508.539333	1152371.725839	43.397543
3508.390628	1152205.711194	43.402548
3508.826795	1152031.453566	43.407553
3508.565081	1151865.920157	43.412557
3508.510528	1151702.808940	43.417562
3508.379247	1151553.244049	43.422567
3508.117409	1151392.808305	43.427572
3508.500388	1151218.343179	43.432577
3508.707947	1151063.690411	43.437581
3508.662258	1150894.019405	43.442586
3508.453068	1150724.464551	43.447591
3508.406442	1150567.661185	43.452596
3508.574272	1150393.393571	43.457601
3508.415853	1150239.155666	43.462605
3508.456346	1150056.658981	43.467610
3508.626399	1149911.733013	43.472615
3508.540363	1149755.764332	43.477620
3508.425947	1149590.135128	43.482625
3508.393474	1149436.421255	43.487629
3508.476711	1149260.141103	43.492634
3508.445255	1149107.175204	43.497639
3508.230645	1148941.257951	43.502644
3508.441693	1148777.065173	43.507649
3508.131565	1148625.362632	43.512653
3508.298813	1148465.714365	43.517658
3508.264050	1148294.536887	43.522663
3507.923259	1148137.614938	43.527668
3507.868494	1147989.546818	43.532673
3507.767824	1147842.997991	43.537677
3507.869211	1147689.590122	43.542682
3508.149802	1147532.547833	43.547687
3507.990393	1147385.048475	43.552692
3508.220638	1147229.710992	43.557697
3507.787133	1147075.236308	43.562701
3508.022073	1146906.243531	43.567706
3508.178161	1146756.305641	43.572711
3507.981095	1146603.389167	43.577716
3507.777305	1146450.848442	43.582721
3507.614915	1146297.727864	43.587725
3507.440061	1146155.314296	43.592730
3507.824946	1146013.278581	43.597735
3507.869950	1145877.266064	43.602740
3507.804842	1145721.648521	43.607745
3507.504030	1145573.174000	43.612749
3507.730276	1145417.025578	43.617754
3507.883145	1145271.311451	43.622759
3507.471024	1145136.776987	43.627764
3507.557715	1144980.449064	43.632769
3507.196934	1144838.125386	43.637773
3507.631131	1144685.807784	43.642778
3507.904214	1144546.026238	43.647783
3507.818891	1144388.002679	43.652788
3507.792744	1144231.576382	43.657793
3507.651011	1144109.959893	43.662797
3507.628158	1143954.757391	43.667802
3507.932475	1143807.555771	43.672807
3507.252440	1143664.210075	43.677812
3507.315207	1143519.600305	43.682817
3507.113443	1143381.004006	43.687821
3507.067993	1143242.378330	43.692826
3506.952819	1143106.036376	43.697831
3506.648266	1142973.704974	43.702836
3507.116996	1142835.458101	43.707841
3506.826009	1142704.160881	43.712845
3506.803415	1142566.556911	43.717850
3507.025704	1142433.081998	43.722855
3507.053388	1142308.266431	43.727860
3507.216170	1142182.856602	43.732865
3507.094080	1142049.144188	43.737869
3507.272222	1141905.040354	43.742874
3507.195231	1141771.028935	43.747879
3506.955929	1141635.997455	43.752884
3507.100754	1141502.796402	43.757889
3506.949113	1141380.170181	43.762893
3506.946550	1141240.346663	43.767898
3506.757796	1141103.301171	43.772903
3506.860239	1140971.516688	43.777908
3506.748956	1140844.981899	43.782913
3506.553170	1140721.209255	43.787917
3506.791464	1140584.744101	43.792922
3506.782458	1140467.765640	43.797927
3506.791617	1140338.637278	43.802932
3506.692519	1140200.509991	43.807937
3506.646879	1140083.434194	43.812941
3506.900255	1139960.423731	43.817946
3507.014516	1139832.973650	43.822951
3506.778380	1139708.519769	43.827956
3506.817175	1139556.404281	43.832961
3506.668462	1139433.922274	43.837965
3506.863241	1139308.439085	43.842970
3506.669009	1139176.753698	43.847975
3506.456452	1139051.900909	43.852980
3506.867459	1138924.569907	43.857985
3506.815695	1138804.999383	43.862989
3506.542505	1138680.432542	43.867994
3506.477058	1138554.120184	43.872999
3506.489469	1138435.764584	43.878004
3506.661778	1138298.207374	43.883009
3506.178849	1138184.958203	43.888013
3506.433632	1138065.700178	43.893018
3506.377282	1137934.435796	43.898023
3505.861938	1137815.678664	43.903028
3506.447811	1137696.832430	43.908033
3506.171781	1137583.441401	43.913037
3506.683097	1137466.026183	43.918042
3506.934719	1137331.278702	43.923047
3506.484167	1137214.111254	43.928052
3506.549818	1137082.141146	43.933057
3506.337333	1136974.517718	43.938061
3506.325029	1136838.661934	43.943066
3506.463374	1136722.146148	43.948071
3506.093133	1136615.111060	43.953076
3506.494571	1136491.805835	43.958081
3506.454384	1136368.760377	43.963085
3506.588307	1136251.095591	43.968090
3506.747268	1136125.258114	43.973095
3506.707086	1136005.147769	43.978100
3506.356570	1135867.898500	43.983105
3506.468298	1135755.733931	43.988109
3506.272839	1135640.958655	43.993114
3506.549074	1135523.539188	43.998119
3506.388483	1135392.893817	44.003124
3506.252331	1135270.028618	44.008129
3505.789731	1135158.040975	44.013133
3506.426199	1135041.026364	44.018138
3506.499566	1134917.643641	44.023143
3506.328382	1134815.478134	44.028148
3506.432610	1134702.247802	44.033153
3506.269211	1134578.801221	44.038157
3506.268667	1134451.620611	44.043162
3506.251716	1134336.217822	44.048167
3505.966738	1134230.830311	44.053172
3506.271067	1134100.931456	44.058177
3506.272626	1133982.668258	44.063181
3506.138065	1133883.233531	44.068186
3506.229431	1133762.670806	44.073191
3506.123562	1133651.162586	44.078196
3506.345492	1133521.168134	44.083201
3505.955059	1133417.586842	44.088205
3506.008964	1133296.544703	44.093210
3506.066963	1133187.944885	44.098215
3505.969318	1133080.983610	44.103220
3506.208289	1132958.858218	44.108225
3506.033707	1132853.995259	44.113229
3505.892087	1132732.877472	44.118234
3506.280865	1132624.496707	44.123239
3506.165450	1132513.061188	44.128244
3506.035422	1132395.639496	44.133249
3505.991106	1132289.318643	44.138253
3505.782461	1132175.230787	44.143258
3506.245734	1132055.043194	44.148263
3505.768338	1131952.397909	44.153268
3506.309104	1131833.522938	44.158273
3506.197673	1131731.098197	44.163277
3505.717775	1131615.237393	44.168282
3506.064040	1131500.948643	44.173287
3505.989506	1131392.333971	44.178292
3506.062625	1131276.849902	44.183297
3505.975272	1131181.443547	44.188301
3505.871974	1131061.136732	44.193306
3506.211174	1130964.420667	44.198311
3505.901079	1130853.267555	44.203316
3505.886060	1130737.881350	44.208321
3505.618680	1130627.096673	44.213325
3505.666068	1130516.257847	44.218330
3505.625924	1130405.906406	44.223335
3505.720954	1130298.762361	44.228340
3505.852839	1130191.705149	44.233345
3505.840716	1130091.228713	44.238349
3505.396078	1129974.280666	44.243354
3506.081494	1129873.685243	44.248359
3505.590597	1129765.010850	44.253364
3505.479274	1129666.348997	44.258369
3505.881739	1129567.315488	44.263373
3505.711674	1129454.303742	44.268378
3505.755513	1129350.476573	44.273383
3505.515403	1129249.071044	44.278388
3505.698362	1129134.948541	44.283393
3505.723238	1129036.632898	44.288397
3505.440821	1128932.280827	44.293402
3505.580019	1128837.365616	44.298407
3505.663069	1128738.559473	44.303412
3505.943406	1128626.692086	44.308417
3505.688046	1128519.284675	44.313421
3505.755577	1128413.248282	44.318426
3505.813587	1128295.800196	44.323431
3505.730913	1128196.250544	44.328436
3505.924741	1128084.956600	44.333441
3505.602495	1127974.886512	44.338445
3505.530269	1127870.954514	44.343450
3505.346681	1127774.837226	44.348455
3505.342813	1127675.264857	44.353460
3505.001759	1127562.621532	44.358465
3505.145374	1127473.768088	44.363469
3505.244392	1127385.110726	44.368474
3505.190058	1127281.544720	44.373479
3505.007976	1127183.799629	44.378484
3505.242965	1127087.981462	44.383489
3505.119392	1127014.097328	44.388493
3504.844738	1126913.033458	44.393498
3505.198646	1126812.339747	44.398503
3504.776108	1126727.657245	44.403508
3505.174888	1126632.564887	44.408513
3504.984683	1126539.280077	44.413517
3505.006973	1126445.863510	44.418522
3505.064158	1126343.402420	44.423527
3504.470736	1126258.930865	44.428532
3505.005987	1126169.325275	44.433537
3504.919710	1126100.749669	44.438541
3505.156535	1125999.203703	44.443546
3505.213086	1125906.533118	44.448551
3505.070311	1125822.170691	44.453556
3505.165793	1125707.798923	44.458561
3505.404520	1125636.404782	44.463565
3505.217428	1125531.209245	44.468570
3505.348441	1125450.982116	44.473575
3505.070005	1125350.745537	44.478580
3505.404533	1125242.128294	44.483585
3504.939461	1125154.192772	44.488589
3505.185710	1125065.187142	44.493594
3505.152307	1124970.136337	44.498599
3505.034338	1124867.485436	44.503604
3504.864012	1124777.116295	44.508609
3504.869562	1124692.711572	44.513613
3504.485493	1124611.890556	44.518618
3504.687836	1124519.742821	44.523623
3504.696195	1124435.333564	44.528628
3504.918079	1124349.555517	44.533633
3505.038639	1124272.738280	44.538637
3504.690225	1124176.488074	44.543642
3505.285617	1124072.943069	44.548647
3505.042519	1123992.755633	44.553652
3505.051639	1123896.727006	44.558657
3504.923715	1123810.141362	44.563661
3504.976801	1123723.048629	44.568666
3505.228241	1123618.980426	44.573671
3505.051042	1123542.296895	44.578676
3505.008562	1123452.169792	44.583681
3505.194929	1123368.856507	44.588685
3504.862547	1123266.305297	44.593690
3505.122815	1123167.176338	44.598695
3504.992809	1123090.288171	44.603700
3505.052613	1122996.614654	44.608705
3505.087035	1122910.653996	44.613709
3504.856927	1122802.936826	44.618714
3504.931507	1122711.730845	44.623719
3504.884846	1122628.920362	44.628724
3504.920688	1122545.714225	44.633729
3504.797441	1122453.679658	44.638733
3504.476738	1122363.199207	44.643738
3504.549521	1122283.219656	44.648743
3504.669151	1122203.231193	44.653748
3504.695490	1122105.644292	44.658753
3504.684313	1122044.620446	44.663757
3504.506033	1121954.204813	44.668762
3504.299797	1121862.649759	44.673767
3504.568481	1121797.863900	44.678772
3504.405981	1121713.630171	44.683777
3504.668475	1121633.038383	44.688781
3504.337507	1121540.451019	44.693786
3504.641286	1121455.850793	44.698791
3504.698526	1121391.570910	44.703796
3504.414047	1121313.254356	44.708801
3504.540666	1121240.010768	44.713805
3504.479051	1121140.611571	44.718810
3504.703469	1121062.112303	44.723815
3504.920252	1120992.564134	44.728820
3504.571884	1120906.062926	44.733825
3504.282015	1120822.502698	44.738829
3504.576179	1120732.845623	44.743834
3504.822146	1120647.861226	44.748839
3504.677486	1120563.415968	44.753844
3504.918098	1120475.096627	44.758849
3504.624915	1120408.005656	44.763853
3504.707216	1120327.995281	44.768858
3504.776985	1120236.557379	44.773863
3504.387093	1120164.241252	44.778868
3504.648352	1120075.054763	44.783873
3504.892170	1119994.631842	44.788877
3504.668436	1119903.427065	44.793882
3504.561242	1119812.582515	44.798887
3504.643505	1119733.610942	44.803892
3504.708758	1119653.593287	44.808897
3504.434878	1119577.535476	44.813901
3504.387158	1119490.771347	44.818906
3504.682462	1119412.140942	44.823911
3504.286826	1119343.624712	44.828916
3504.418649	1119257.589251	44.833921
3504.315999	1119178.830451	44.838925
3504.221247	1119109.690135	44.843930
3504.560931	1119026.283912	44.848935
3504.376697	1118965.824969	44.853940
3504.762563	1118861.832522	44.858945
3504.833697	1118790.565015	44.863949
3504.192349	1118708.744352	44.868954
3504.208838	1118625.099317	44.873959
3504.257073	1118552.879762	44.878964
3504.333821	1118469.508170	44.883969
3504.466075	1118413.563733	44.888973
3504.478321	1118329.152618	44.893978
3504.454422	1118249.795549	44.898983
3504.338877	1118174.549155	44.903988
3504.590146	1118098.860192	44.908993
3504.598578	1118009.109270	44.913997
3504.580633	1117924.982584	44.919002
3504.548787	1117847.526417	44.924007
3504.146619	1117779.753454	44.929012
3504.289193	1117698.359903	44.934017
3504.534769	1117617.234001	44.939021
3504.142512	1117543.929981	44.944026
3504.331694	1117466.813042	44.949031
3504.340177	1117414.594707	44.954036
3504.581641	1117327.271436	44.959041
3504.293877	1117248.705292	44.964045
3504.180261	1117177.732612	44.969050
3504.456909	1117095.640783	44.974055
3504.321984	1117022.287235	44.979060
3504.461410	1116944.027440	44.984065
3504.395656	1116868.563897	44.989069
3504.244508	1116783.488247	44.994074
3504.341218	1116703.230707	44.999079
3504.299743	1116641.673694	45.004084
3504.272863	1116558.003506	45.009089
3504.546695	1116493.915009	45.014093
3504.301849	1116421.619674	45.019098
3504.244395	1116334.234145	45.024103
3504.205933	1116266.477419	45.029108
3503.930563	1116196.280830	45.034113
3504.185293	1116118.943080	45.039117
3503.976596	1116051.402291	45.044122
3504.187425	1115975.499370	45.049127
3503.648662	1115907.343935	45.054132
3504.094051	1115831.876919	45.059137
3504.176143	1115766.572209	45.064141
3503.791431	1115702.773345	45.069146
3504.323707	1115635.963141	45.074151
3503.947537	1115565.107649	45.079156
3504.123640	1115487.201818	45.084161
3503.895352	1115425.470955	45.089165
3503.831694	1115358.278828	45.094170
3504.140777	1115278.060291	45.099175
3503.830829	1115221.011442	45.104180
3503.792481	1115147.520987	45.109185
3504.172240	1115089.403873	45.114189
3503.816854	1115019.109705	45.119194
3504.205698	1114940.684248	45.124199
3504.000061	1114873.414096	45.129204
3504.098017	1114803.042430	45.134209
3504.211619	1114741.342712	45.139213
3504.049255	1114666.722076	45.144218
3504.028983	1114591.028291	45.149223
3503.760019	1114532.058611	45.154228
3503.701229	1114470.574845	45.159233
3504.099357	1114408.824442	45.164237
3504.150068	1114341.028686	45.169242
3504.306557	1114266.349965	45.174247
3503.913497	1114188.709695	45.179252
3503.564280	1114109.726238	45.184257
3504.280845	1114048.872707	45.189261
3504.093748	1113991.123101	45.194266
3504.200845	1113901.668503	45.199271
3503.987090	1113849.642726	45.204276
3504.268467	1113776.080817	45.209281
3504.002007	1113703.180244	45.214285
3504.106097	1113626.784897	45.219290
3503.968832	1113557.961306	45.224295
3503.925604	1113511.816205	45.229300
3503.932793	1113426.565819	45.234305
3504.102083	1113366.176123	45.239309
3503.635790	1113293.207528	45.244314
3504.115480	1113221.035755	45.249319
3504.016251	1113167.840161	45.254324
3503.682498	1113088.648389	45.259329
3504.113197	1113029.546948	45.264333
3504.042013	1112961.658472	45.269338
3504.273475	1112880.653951	45.274343
3504.148298	1112819.352926	45.279348
3504.154451	1112740.576878	45.284353
3503.962903	1112679.762038	45.289357
3503.876754	1112603.478828	45.294362
3503.835527	1112539.585722	45.299367
3503.619137	1112486.974914	45.304372
3503.859608	1112417.502232	45.309377
3504.038169	1112342.411601	45.314381
3503.655180	1112288.109492	45.319386
3503.937272	1112219.676556	45.324391
3504.063611	1112163.858616	45.329396
3504.148359	1112084.392332	45.334401
3504.209379	1112010.460998	45.339405
3503.730994	1111945.678990	45.344410
3504.104546	1111875.700463	45.349415
3503.939629	1111809.529787	45.354420
3504.112223	1111731.379223	45.359425
3504.481730	1111673.417603	45.364429
3504.224268	1111600.296188	45.369434
3503.891017	1111523.942941	45.374439
3503.520430	1111465.242439	45.379444
3503.513410	1111403.810390	45.384449
3503.948499	1111342.304826	45.389453
3503.605168	1111270.433191	45.394458
3503.964028	1111199.494317	45.399463
3503.673019	1111153.655939	45.404468
3503.717316	1111090.017690	45.409473
3503.706648	1111024.956732	45.414477
3503.489650	1110958.879548	45.419482
3503.806426	1110896.434352	45.424487
3503.607301	1110835.981476	45.429492
3503.553927	1110779.701731	45.434497
3503.678333	1110723.869147	45.439501
3503.672984	1110657.944214	45.444506
3503.922868	1110591.213171	45.449511
3503.906457	1110522.426150	45.454516
3503.670169	1110460.066973	45.459521
3504.154304	1110398.160892	45.464525
3503.822306	1110330.377504	45.469530
3503.709527	1110261.412186	45.474535
3503.760333	1110209.498358	45.479540
3503.826871	1110152.715221	45.484545
3503.465070	1110072.529388	45.489549
3503.500559	1110017.658287	45.494554
3503.685382	1109946.159029	45.499559
3503.901799	1109896.123292	45.504564
3503.695352	1109837.282529	45.509569
3503.427140	1109773.584736	45.514573
3503.340830	1109699.836710	45.519578
3503.510621	1109647.516160	45.524583
3503.333211	1109618.917862	45.529588
3503.378520	1109552.112189	45.534593
3503.695926	1109487.074003	45.539597
3503.542748	1109432.227998	45.544602
3503.607105	1109377.441036	45.549607
3503.606533	1109314.743450	45.554612
3503.516682	1109247.669963	45.559617
3503.719658	1109188.563801	45.564621
3503.498022	1109138.020558	45.569626
3503.534914	1109075.791185	45.574631
3503.486273	1109023.786849	45.579636
3503.532559	1108955.828374	45.584641
3503.294664	1108899.177572	45.589645
3503.295027	1108847.163456	45.594650
3503.668456	1108785.543374	45.599655
3503.215832	1108733.411882	45.604660
3503.327160	1108665.343583	45.609665
3503.431097	1108614.360023	45.614669
3503.319328	1108558.257516	45.619674
3503.448192	1108502.210237	45.624679
3503.282678	1108452.319418	45.629684
3503.291004	1108402.304058	45.634689
3503.500123	1108336.506222	45.639693
3503.338755	1108290.144800	45.644698
3503.273409	1108235.653915	45.649703
3503.370032	1108174.167873	45.654708
3503.422749	1108120.992697	45.659713
3503.732056	1108066.915660	45.664717
3503.596013	1108013.579605	45.669722
3503.579050	1107939.414192	45.674727
3503.380772	1107890.764477	45.679732
3503.141313	1107831.907190	45.684737
3503.481623	1107766.176233	45.689741
3503.060301	1107730.066831	45.694746
3503.111539	1107672.591810	45.699751
3503.412749	1107626.530321	45.704756
3503.464066	1107574.495506	45.709761
3503.739647	1107519.845759	45.714765
3503.313571	1107459.869582	45.719770
3503.751490	1107400.609624	45.724775
3503.474139	1107343.567065	45.729780
3503.459289	1107284.189463	45.734785
3503.398283	1107232.933579	45.739789
3503.405827	1107177.560760	45.744794
3503.497080	1107114.726934	45.749799
3503.342420	1107069.976875	45.754804
3503.476087	1106999.783471	45.759809
3503.375976	1106946.621861	45.764813
3503.066312	1106874.113008	45.769818
3503.344098	1106750.713222	45.774823
3503.403457	1106592.305827	45.779828
3502.995514	1106356.056845	45.784833
3503.532782	1106064.831662	45.789837
3503.189011	1105697.340318	45.794842
3503.118428	1105277.634772	45.799847
3502.944094	1104789.145997	45.804852
3502.819094	1104247.495508	45.809857
3502.973306	1103629.128676	45.814861
3502.700582	1102959.741188	45.819866
3502.811078	1102205.831344	45.824871
3502.689695	1101404.929097	45.829876
3502.247411	1100520.227430	45.834881
3502.155688	1099559.605328	45.839885
3501.832744	1098541.190780	45.844890
3502.027975	1097445.030084	45.849895
3501.739207	1096272.484809	45.854900
3501.473207	1095016.724056	45.859905
3501.424751	1093687.420234	45.864909
3501.119967	1092302.403730	45.869914
3501.032173	1090818.846106	45.874919
3501.012082	1089263.128405	45.879924
3500.491235	1087612.957812	45.884929
3500.368188	1085894.745693	45.889933
3499.983062	1084099.140929	45.894938
3499.993841	1082208.599433	45.899943
3499.836163	1080244.991528	45.904948
3499.328309	1078201.454387	45.909953
3499.084548	1076075.973586	45.914957
3498.702995	1073862.373140	45.919962
3498.143160	1071556.613882	45.924967
3497.933881	1069182.432249	45.929972
3497.336886	1066735.534311	45.934977
3497.139483	1064182.207888	45.939981
3496.755166	1061561.586163	45.944986
3496.250827	1058857.671165	45.949991
3496.010262	1056089.938332	45.954996
3495.533577	1053221.255428	45.960001
3495.029896	1050266.000191	45.965005
3494.477107	1047244.599679	45.970010
3494.157367	1044130.729975	45.975015
3493.787786	1040936.461012	45.980020
3493.127642	1037653.478726	45.985025
3492.778865	1034290.141307	45.990029
3492.031855	1030855.427527	45.995034
3491.512924	1027332.832919	46.000039
3491.250792	1023725.584075	46.005044
3490.151187	1020045.245248	46.010049
3490.258556	1016273.190883	46.015053
3489.163671	1012412.261750	46.020058
3488.904520	1008479.051416	46.025063
3487.986907	1004453.333614	46.030068
3487.215446	1000340.624979	46.035073
3486.958152	996165.521531	46.040077
3486.105842	991898.930024	46.045082
3485.237631	987535.581869	46.050087
3484.727429	983103.221857	46.055092
3484.086034	978599.727442	46.060097
3483.541558	973993.611377	46.065101
3482.576323	969314.179434	46.070106
3482.063106	964537.024498	46.075111
3481.038789	959681.287325	46.080116
3480.198685	954746.274373	46.085121
3479.716951	949850.820635	46.090125
3478.395325	944868.096373	46.095130
3477.550088	939796.781074	46.100135
3476.830632	934671.955032	46.105140
3475.593780	929457.301651	46.110145
3474.673369	924157.476289	46.115149
3473.525409	918770.545631	46.120154
3472.887680	913316.234695	46.125159
3471.693157	907763.904429	46.130164
3470.668397	902138.505933	46.135169
3469.962788	896432.612761	46.140173
3468.714134	890644.549182	46.145178
3467.728989	884763.254537	46.150183
3466.600033	878821.650245	46.155188
3465.345892	872769.644127	46.160193
3464.298530	866641.414883	46.165197
3462.711711	860448.606559	46.170202
3461.654311	854170.682178	46.175207
3460.749342	847810.651085	46.180212
3458.965579	841358.280870	46.185217
3458.129820	834829.780655	46.190221
3457.215461	828231.098776	46.195226
3456.025636	821537.789334	46.200231
3454.694277	814761.252073	46.205236
3453.320968	807905.785043	46.210241
3452.238018	800953.929817	46.215245
3450.655244	793934.571023	46.220250
3449.157124	786831.002747	46.225255
3448.005651	779641.128324	46.230260
3446.257207	772378.516575	46.235265
3445.125589	765023.247571	46.240269
3443.644422	757617.543379	46.245274
3442.421710	750115.430174	46.250279
3440.774405	742510.097452	46.255284
3439.186396	734824.722305	46.260289
3437.857912	727057.646973	46.265293
3435.977749	719239.274492	46.270298
3434.964158	711329.107697	46.275303
3433.339821	703334.738799	46.280308
3431.513058	695250.748934	46.285313
3429.742586	687099.810096	46.290317
3427.769752	678873.573349	46.295322
3426.531931	670562.420863	46.300327
3424.874729	662177.019691	46.305332
3422.645927	653722.518792	46.310337
3421.170495	645183.945684	46.315341
3418.706604	636590.379410	46.320346
3417.105710	627923.828095	46.325351
3415.871240	619182.274069	46.330356
3413.679697	610359.872517	46.335361
3411.941295	601449.261847	46.340365
3409.674715	592487.926230	46.345370
3407.620185	583446.965147	46.350375
3405.656179	574342.424727	46.355380
3403.772902	565168.582854	46.360385
3401.896006	555918.005154	46.365389
3399.534224	546608.423613	46.370394
3397.598627	537222.982269	46.375399
3395.887345	527773.851530	46.380404
3393.308281	518246.004697	46.385409
3391.381956	508662.424210	46.390413
3388.941475	499007.954756	46.395418
3386.885777	489292.326203	46.400423
3384.537833	479499.125364	46.405428
3382.035884	469675.004901	46.410433
3379.861547	459760.522020	46.415437
3377.241965	449790.351752	46.420442
3374.467143	439763.502625	46.425447
3372.036562	429693.166115	46.430452
3368.698415	419540.269855	46.435457
3366.845254	409343.086491	46.440461
3364.288661	399116.369460	46.445466
3361.527514	388822.680312	46.450471
3358.944790	378469.634916	46.455476
3355.916192	368076.248924	46.460481
3353.172093	357626.466341	46.465485
3350.137684	347137.082548	46.470490
3347.238043	336605.611889	46.475495
3344.196103	326032.004761	46.480500
3340.886164	315420.648113	46.485505
3338.112811	304759.412088	46.490509
3334.678241	294077.750593	46.495514
3331.403255	283348.545708	46.500519
3327.996646	272585.940530	46.505524
3324.464856	261812.799047	46.510529
3321.382602	250995.917540	46.515533
3317.540505	240157.529324	46.520538
3313.934385	229242.218859	46.525543
3310.170593	218327.740721	46.530548
3306.169746	207422.025588	46.535553
3302.324045	196513.639108	46.540557
3298.382950	185617.665451	46.545562
3294.405182	174688.311425	46.550567
3289.811404	163757.572507	46.555572
3285.067622	152828.517954	46.560577
3280.767114	141924.838043	46.565581
3275.828846	131009.316904	46.570586
3270.587165	120121.424587	46.575591
3265.447080	109269.627498	46.580596
3259.872401	98447.011832	46.585601
3253.849235	87650.664280	46.590605
3247.879374	76912.088645	46.595610
3241.244174	66226.925943	46.600615
3234.524157	55624.847685	46.605620
3226.723929	45095.644562	46.610625
3218.367627	34682.840395	46.615629
3207.625529	24444.438232	46.620634
3168.481957	15130.274914	46.625639
3099.209182	7029.036612	46.630644
2985.737286	1018.663145	46.635649
2731.395703	416.575753	46.640653
2570.550010	433.197022	46.645658
2539.851631	424.329759	46.650663
2601.379598	405.876127	46.655668
2699.721417	377.223848	46.660673
2789.604516	371.546576	46.665677
2847.817479	368.156212	46.670682
2871.623464	379.129844	46.675687
2871.495900	378.222062	46.680692
2858.447177	390.660983	46.685697
2843.229858	362.994921	46.690701
2831.662472	365.657582	46.695706
2823.809363	358.447258	46.700711
2820.308887	353.641903	46.705716
2818.806724	378.730704	46.710721
2818.327435	363.641344	46.715725
2817.574916	355.504307	46.720730
2815.824932	353.302043	46.725735
2813.511581	347.473733	46.730740
2810.132187	353.343967	46.735745
2807.182681	352.649643	46.740749
2803.989586	356.302800	46.745754
2800.936541	339.893011	46.750759
2798.004258	341.077658	46.755764
2794.632699	352.534607	46.760769
2791.534593	336.444706	46.765773
2787.915523	346.312922	46.770778
2785.186870	341.691313	46.775783
2782.179303	330.690481	46.780788
2779.100155	335.040918	46.785793
2775.983572	329.309044	46.790797
2772.662560	332.127932	46.795802
2769.469086	334.790337	46.800807
2766.141990	328.004976	46.805812
2762.986260	329.803426	46.810817
2759.477091	327.027264	46.815821
2756.142544	331.957897	46.820826
2752.505458	331.179343	46.825831
2749.895392	318.385300	46.830836
2745.949713	327.995214	46.835841
2742.889248	323.095560	46.840845
2739.440494	322.006662	46.845850
2735.847230	329.315685	46.850855
2732.729485	320.891747	46.855860
2729.454478	322.325504	46.860865
2726.066080	318.273827	46.865869
2723.171537	317.722902	46.870874
2719.545685	316.450408	46.875879
2716.375919	313.252487	46.880884
2712.398677	324.021223	46.885889
2709.243981	325.429923	46.890893
2705.964393	310.721832	46.895898
2702.096577	318.768314	46.900903
2698.762637	305.629469	46.905908
2695.540268	307.855760	46.910913
2692.444330	312.331129	46.915917
2688.614582	314.383889	46.920922
2685.243283	298.337949	46.925927
2682.060224	295.050488	46.930932
2678.894310	312.429608	46.935937
2675.416507	310.539890	46.940941
2671.522880	293.410298	46.945946
2667.672469	307.125359	46.950951
2664.695131	297.411058	46.955956
2660.932088	298.357138	46.960961
2657.515511	301.855297	46.965965
2654.567833	300.326385	46.970970
2651.371215	303.270721	46.975975
2648.030079	288.590888	46.980980
2643.781771	299.224969	46.985985
2640.633037	304.345500	46.990989
2636.710395	291.217050	46.995994
2633.336693	294.314997	47.000999
2630.841041	294.897720	47.006004
2627.135389	287.103641	47.011009
2623.027979	288.917486	47.016013
2619.932611	307.527180	47.021018
2616.465701	295.462699	47.026023
2612.741271	291.649502	47.031028
2609.131362	300.451925	47.036033
2606.445361	292.481834	47.041037
2602.814638	298.539876	47.046042
2599.390727	285.289857	47.051047
2596.005281	286.910975	47.056052
2592.528774	298.968419	47.061057
2588.793781	290.461166	47.066061
2585.165653	286.689820	47.071066
2581.719837	299.733026	47.076071
2578.312743	283.874994	47.081076
2575.294022	284.092033	47.086081
2571.606689	283.746576	47.091085
2567.926231	288.658141	47.096090
2564.518624	283.276758	47.101095
2561.795237	288.076288	47.106100
2557.756523	284.572639	47.111105
2554.142487	289.937047	47.116109
2550.055944	283.838307	47.121114
2546.185193	267.551344	47.126119
2543.496582	277.126281	47.131124
2540.220435	288.769187	47.136129
2537.115809	274.314443	47.141133
2533.457869	278.461953	47.146138
2530.035395	285.598833	47.151143
2526.602397	286.728911	47.156148
2522.877202	281.714142	47.161153
2519.075671	283.942772	47.166157
2515.642121	289.288187	47.171162
2512.153342	275.556328	47.176167
2508.827379	275.720467	47.181172
2505.051983	290.807267	47.186177
2502.215348	268.870169	47.191181
2498.570327	276.828082	47.196186
2494.784222	281.382002	47.201191
2491.911000	270.944937	47.206196
2488.048879	270.693852	47.211201
2484.344491	274.037585	47.216205
2481.157230	267.458519	47.221210
2477.457756	265.181228	47.226215
2474.258562	267.540224	47.231220
2470.130946	274.825072	47.236225
2467.243972	271.855202	47.241229
2463.943470	264.940540	47.246234
2460.224292	273.986653	47.251239
2456.620857	264.559719	47.256244
2452.766077	264.565924	47.261249
2449.590178	267.991027	47.266253
2446.105068	264.806074	47.271258
2442.457300	268.351318	47.276263
2439.585926	254.862711	47.281268
2436.040744	265.766364	47.286273
2432.591677	265.303547	47.291277
2429.037743	261.877488	47.296282
2424.986929	251.666336	47.301287
2421.729842	250.164081	47.306292
2418.255511	262.372042	47.311297
2414.467027	261.457911	47.316301
2411.334999	260.302732	47.321306
2407.841573	254.179876	47.326311
2404.695450	252.838097	47.331316
2401.024789	262.875919	47.336321
2397.309324	247.511863	47.341325
2393.535629	254.716074	47.346330
2390.103334	262.010199	47.351335
2386.753892	249.403239	47.356340
2382.974575	261.393851	47.361345
2379.799777	257.313843	47.366349
2376.512116	248.727737	47.371354
2373.118322	258.979770	47.376359
2369.524069	258.489032	47.381364
2365.815483	254.620582	47.386369
2362.526373	256.617677	47.391373
2359.001725	255.846230	47.396378
2355.046286	261.161946	47.401383
2352.090331	255.400356	47.406388
2348.579475	262.856425	47.411393
2345.111434	261.170962	47.416397
2341.523007	260.193685	47.421402
2337.719734	254.466675	47.426407
2334.446613	251.037370	47.431412
2330.795152	257.695608	47.436417
2327.598307	261.064029	47.441421
2324.108970	259.520603	47.446426
2320.179411	265.596366	47.451431
2317.147655	252.528017	47.456436
2313.522745	258.976775	47.461441
2310.014727	253.504259	47.466445
2306.655701	256.850700	47.471450
2302.753650	250.136856	47.476455
2299.869791	254.584377	47.481460
2296.016040	262.335078	47.486465
2292.380205	262.637532	47.491469
2289.180602	255.548373	47.496474
2285.196787	257.751039	47.501479
2282.064070	258.870569	47.506484
2278.529322	257.228499	47.511489
2275.104367	246.615392	47.516493
2271.930051	256.379607	47.521498
2268.030800	258.011218	47.526503
2264.896063	245.383621	47.531508
2261.002547	255.220089	47.536513
2257.632859	253.546861	47.541517
2254.044303	244.610987	47.546522
2250.397159	260.202730	47.551527
2247.249604	252.390139	47.556532
2243.800038	247.803629	47.561537
2240.242037	249.221907	47.566541
2236.249971	251.980904	47.571546
2232.944042	252.060074	47.576551
2229.888321	246.123012	47.581556
2226.074849	247.216035	47.586561
2222.750659	254.356143	47.591565
2219.103384	238.777042	47.596570
2215.068684	245.316216	47.601575
2212.118738	233.223977	47.606580
2208.529794	247.884470	47.611585
2205.480343	250.206836	47.616589
2202.095647	247.214599	47.621594
2198.493135	241.617738	47.626599
2194.816650	241.968085	47.631604
2190.980097	244.321328	47.636609
2187.581003	251.245116	47.641613
2183.863845	248.332882	47.646618
2179.985649	247.697973	47.651623
2177.061220	227.113107	47.656628
2173.625579	244.931978	47.661633
2170.496883	233.804019	47.666637
2166.811221	230.000960	47.671642
2163.159624	240.871240	47.676647
2159.870919	234.321609	47.681652
2156.071846	238.532117	47.686657
2152.945537	241.182092	47.691661
2149.334682	234.737695	47.696666
2145.343982	236.665524	47.701671
2142.232900	234.716274	47.706676
2138.552079	241.854855	47.711681
2135.291133	231.072918	47.716685
2132.109859	234.459166	47.721690
2128.042332	239.221459	47.726695
2124.545467	221.752619	47.731700
2121.006837	236.321762	47.736705
2117.670823	240.908938	47.741709
2114.468423	235.714057	47.746714
2110.658056	239.955060	47.751719
2107.019796	241.255622	47.756724
2103.637592	236.140029	47.761729
2100.006770	233.858915	47.766733
2096.742378	225.925004	47.771738
2092.989758	232.459431	47.776743
2089.955995	230.930060	47.781748
2086.087617	223.431318	47.786753
2082.919205	228.937371	47.791757
2079.377551	228.986039	47.796762
2075.613791	231.216834	47.801767
2072.020060	225.558518	47.806772
2068.753831	238.859994	47.811777
2065.053118	232.488873	47.816781
2061.703169	227.486174	47.821786
2058.061728	238.975367	47.826791
2055.008086	232.935349	47.831796
2051.117665	236.368071	47.836801
2047.627637	231.189692	47.841805
2044.248841	228.450308	47.846810
2040.717119	231.827217	47.851815
2037.339061	224.723046	47.856820
2033.441606	237.109931	47.861825
2029.959749	226.805986	47.866829
2026.601001	235.527308	47.871834
2023.156274	239.691066	47.876839
2019.719538	226.227109	47.881844
2016.122618	225.866916	47.886849
2012.624287	229.052262	47.891853
2009.452847	223.661823	47.896858
2005.902309	219.570191	47.901863
2002.162790	229.154339	47.906868
1998.671259	240.298289	47.911873
1994.804077	227.563495	47.916877
1991.486628	224.419983	47.921882
1988.006914	225.642948	47.926887
1984.484595	229.444823	47.931892
1981.405794	229.818616	47.936897
1977.849601	222.136732	47.941901
1974.208177	230.632312	47.946906
1970.896934	227.737387	47.951911
1967.369566	212.324865	47.956916
1963.561908	218.077692	47.961921
1960.019090	219.500007	47.966925
1956.836195	225.235307	47.971930
1953.181975	215.945232	47.976935
1949.858468	219.636974	47.981940
1946.183311	224.016160	47.986945
1942.611798	222.088403	47.991949
1939.587994	218.163357	47.996954
1935.190942	229.962918	48.001959
1931.938543	226.514509	48.006964
1928.396652	222.377786	48.011969
1925.013472	225.614910	48.016973
1921.910480	210.594316	48.021978
1917.786213	216.188667	48.026983
1915.081207	221.791569	48.031988
1911.075848	209.194972	48.036993
1907.736049	211.167963	48.041997
1904.353098	221.498060	48.047002
1900.622139	225.415093	48.052007
1897.087774	213.916388	48.057012
1893.646585	213.317269	48.062017
1890.544845	211.538453	48.067021
1887.230031	215.981337	48.072026
1883.194635	220.206689	48.077031
1879.792225	221.078658	48.082036
1875.938981	220.420459	48.087041
1872.218818	218.138817	48.092045
1869.041742	219.383531	48.097050
1865.698297	222.924695	48.102055
1862.597481	219.145379	48.107060
1858.779302	216.644324	48.112065
1855.086194	213.853798	48.117069
1851.462213	209.814521	48.122074
1847.937566	226.695422	48.127079
1844.365321	213.269826	48.132084
1841.360640	214.588810	48.137089
1837.789218	226.134103	48.142093
1834.339169	217.417841	48.147098
1830.450280	218.726640	48.152103
1826.976684	217.966071	48.157108
1823.386149	215.620548	48.162113
1820.209770	211.816330	48.167117
1816.710060	221.149662	48.172122
1813.068065	221.698332	48.177127
1809.400423	219.744772	48.182132
1806.330889	220.156769	48.187137
1802.312616	222.982463	48.192141
1799.055185	220.010573	48.197146
1795.651088	218.980764	48.202151
1792.330883	215.970006	48.207156
1788.766002	222.454351	48.212161
1784.929652	211.042638	48.217165
1781.644194	211.435616	48.222170
1777.695206	220.011814	48.227175
1774.715251	209.390713	48.232180
1771.071800	208.755375	48.237185
1767.561702	218.047621	48.242189
1764.570335	212.330147	48.247194
1760.515174	226.717957	48.252199
1757.451695	212.277945	48.257204
1753.747134	215.030788	48.262209
1750.282798	215.022365	48.267213
1746.732022	207.380078	48.272218
1742.841550	222.179837	48.277223
1739.385032	210.190496	48.282228
1735.856633	206.993525	48.287233
1732.457566	213.969956	48.292237
1729.117581	215.592432	48.297242
1725.720334	212.292433	48.302247
1722.089593	202.833186	48.307252
1718.737884	207.232404	48.312257
1715.146698	213.689351	48.317261
1711.741875	208.097149	48.322266
1707.846517	213.918628	48.327271
1704.581151	222.707821	48.332276
1701.263025	216.261653	48.337281
1697.336602	220.929548	48.342285
1694.379250	215.144734	48.347290
1690.302549	210.956595	48.352295
1687.003318	212.525503	48.357300
1683.379335	198.892701	48.362305
1680.067023	202.475861	48.367309
1676.710456	206.917038	48.372314
1673.200859	206.167420	48.377319
1669.330004	205.393163	48.382324
1665.869394	201.266557	48.387329
1662.474681	193.163599	48.392333
1659.509939	195.156298	48.397338
1655.599555	198.886007	48.402343
1651.875168	202.647968	48.407348
1648.704814	200.673900	48.412353
1645.214642	199.939441	48.417357
1641.589929	204.322278	48.422362
1637.886561	210.027659	48.427367
1634.561009	201.301533	48.432372
1630.785062	199.276167	48.437377
1627.352225	202.434497	48.442381
1623.937176	201.084271	48.447386
1620.507447	210.133044	48.452391
1616.971388	200.715952	48.457396
1613.123806	200.906392	48.462401
1609.677260	206.728339	48.467405
1606.716909	203.546910	48.472410
1603.068461	200.428128	48.477415
1600.208658	214.394687	48.482420
1596.241332	199.964830	48.487425
1592.304164	202.393871	48.492429
1589.045451	209.308523	48.497434
1585.096412	201.470913	48.502439
1581.956705	198.005468	48.507444
1578.583835	199.921611	48.512449
1575.133196	198.881538	48.517453
1571.752848	199.578644	48.522458
1567.384318	194.666169	48.527463
1564.429133	205.565867	48.532468
1560.989003	198.725757	48.537473
1557.184618	203.959201	48.542477
1554.310484	197.046409	48.547482
1550.421572	199.052364	48.552487
1547.337401	192.131127	48.557492
1543.720234	197.219929	48.562497
1539.703997	199.707921	48.567501
1536.415637	191.066285	48.572506
1532.885299	196.258655	48.577511
1529.339168	196.582794	48.582516
1526.151185	195.324778	48.587521
1522.432244	189.904393	48.592525
1518.959377	198.521990	48.597530
1515.353785	209.135307	48.602535
1512.196148	187.986216	48.607540
1508.718437	187.713748	48.612545
1504.914314	203.537290	48.617549
1501.220345	190.282475	48.622554
1497.361416	190.175037	48.627559
1494.410704	192.551329	48.632564
1491.134769	189.544767	48.637569
1487.474284	186.797701	48.642573
1484.070027	191.652993	48.647578
1480.202068	200.620928	48.652583
1476.829202	196.163454	48.657588
1473.116092	191.621454	48.662593
1469.662718	188.210793	48.667597
1466.867582	187.096036	48.672602
1463.043869	202.959920	48.677607
1459.313919	198.976039	48.682612
1455.957877	198.911017	48.687617
1452.140101	189.928638	48.692621
1448.993859	185.505799	48.697626
1445.350764	187.276098	48.702631
1441.596482	194.238949	48.707636
1438.232942	190.924465	48.712641
1435.176162	186.813417	48.717645
1431.751729	189.439777	48.722650
1428.026796	197.687125	48.727655
1424.196473	187.741588	48.732660
1420.966477	193.600185	48.737665
1417.360323	196.814345	48.742669
1413.720443	196.007536	48.747674
1410.182491	202.495090	48.752679
1406.997453	196.648162	48.757684
1403.499562	195.811313	48.762689
1399.522233	196.096586	48.767693
1396.379568	188.809697	48.772698
1392.675363	197.045944	48.777703
1389.086790	201.826337	48.782708
1385.699872	187.884692	48.787713
1382.345400	198.183726	48.792717
1378.664835	189.482904	48.797722
1375.475820	187.002194	48.802727
1372.046367	182.636004	48.807732
1368.247315	185.510093	48.812737
1364.795749	189.122883	48.817741
1361.517468	189.360178	48.822746
1357.741007	197.567918	48.827751
1354.145106	196.463044	48.832756
1351.018861	195.861044	48.837761
1346.921184	187.188246	48.842765
1343.795105	180.727163	48.847770
1340.313061	195.991296	48.852775
1336.792793	185.513399	48.857780
1333.431492	178.624999	48.862785
1329.688980	195.033420	48.867789
1326.001663	193.322218	48.872794
1322.861967	189.197781	48.877799
1319.411857	185.841020	48.882804
1316.005155	193.957753	48.887809
1311.834316	189.281363	48.892813
1308.901243	191.420708	48.897818
1305.298539	201.697903	48.902823
1301.985147	181.569123	48.907828
1298.499078	186.439577	48.912833
1294.895980	195.536028	48.917837
1291.476711	193.765703	48.922842
1287.536841	189.027823	48.927847
1284.118173	191.793096	48.932852
1280.730688	197.648642	48.937857
1276.905693	179.347676	48.942861
1273.973852	179.436867	48.947866
1270.219158	192.341692	48.952871
1266.633377	187.489143	48.957876
1263.329005	189.636620	48.962881
1259.733325	187.191426	48.967885
1256.137822	182.655595	48.972890
1252.241045	192.929456	48.977895
1249.309118	185.870285	48.982900
1245.900448	182.236901	48.987905
1242.261414	182.499274	48.992909
1238.854410	186.364919	48.997914
1235.422755	189.042483	49.002919
1231.571598	183.916584	49.007924
1228.291676	180.743297	49.012929
1224.242077	178.079259	49.017933
1221.548392	173.889242	49.022938
1217.626602	177.243206	49.027943
1214.118380	183.550127	49.032948
1210.789411	185.398520	49.037953
1207.325254	182.927007	49.042957
1203.980810	175.014815	49.047962
1200.211846	187.051090	49.052967
1196.538978	177.373810	49.057972
1193.100892	180.803222	49.062977
1189.530244	182.236719	49.067981
1186.265947	176.431905	49.072986
1182.499133	179.658590	49.077991
1178.965941	171.975081	49.082996
1175.402008	179.675745	49.088001
1171.873480	184.932102	49.093005
1168.688101	182.664187	49.098010
1165.382873	182.407222	49.103015
1161.656785	172.706295	49.108020
1158.069355	183.784369	49.113025
1154.694134	180.295469	49.118029
1151.624360	184.031096	49.123034
1147.313893	185.684022	49.128039
1143.901270	177.708238	49.133044
1140.677251	174.244700	49.138049
1137.145676	193.120662	49.143053
1133.863916	175.083314	49.148058
1129.930075	179.897638	49.153063
1126.485368	183.313080	49.158068
1123.322568	179.111169	49.163073
1119.183977	179.186650	49.168077
1115.951185	179.155609	49.173082
1112.385176	185.065064	49.178087
1109.050012	175.762622	49.183092
1105.845707	179.498378	49.188097
1102.165465	180.639543	49.193101
1098.877202	172.710541	49.198106
1095.243731	181.380369	49.203111
1091.522725	177.784230	49.208116
1088.202301	185.505406	49.213121
1084.256575	189.022132	49.218125
1080.863811	170.400367	49.223130
1077.424878	180.897244	49.228135
1074.130982	184.687563	49.233140
1070.805373	177.032590	49.238145
1066.735174	179.709204	49.243149
1063.713242	176.614065	49.248154
1060.112939	181.225278	49.253159
1056.658525	168.421847	49.258164
1053.215915	178.442736	49.263169
1049.495327	186.802097	49.268173
1045.830732	170.260990	49.273178
1041.943780	176.363751	49.278183
1038.830579	167.469052	49.283188
1035.860780	170.443469	49.288193
1032.018086	172.286887	49.293197
1028.610447	174.180415	49.298202
1025.077415	171.685844	49.303207
1021.451435	169.758203	49.308212
1018.350257	180.172010	49.313217
1014.392456	169.844108	49.318221
1011.266015	157.384936	49.323226
1007.482714	169.806330	49.328231
1003.734114	175.110936	49.333236
1000.599628	172.474118	49.338241
996.529910	168.255878	49.343245
993.704535	172.355899	49.348250
989.982223	189.473691	49.353255
986.704033	172.160480	49.358260
982.867755	176.745973	49.363265
979.387443	175.483805	49.368269
975.896587	167.634003	49.373274
972.384290	173.489566	49.378279
969.116359	180.187847	49.383284
965.422885	184.206774	49.388289
961.641643	169.672003	49.393293
958.784499	162.555163	49.398298
954.940719	168.331293	49.403303
951.510308	181.333738	49.408308
948.023708	174.219017	49.413313
944.196652	168.509527	49.418317
941.019378	172.030458	49.423322
937.316709	184.841685	49.428327
933.946955	179.337363	49.433332
930.578113	169.334812	49.438337
926.620752	180.757595	49.443341
923.377521	167.380034	49.448346
919.862812	171.797035	49.453351
916.420940	180.535834	49.458356
913.072510	172.893502	49.463361
909.228797	181.677643	49.468365
906.075114	179.649389	49.473370
902.383522	172.765361	49.478375
898.810025	176.024103	49.483380
895.512265	176.309134	49.488385
891.549898	174.171925	49.493389
888.533830	173.464145	49.498394
884.772875	188.687668	49.503399
881.651146	182.766542	49.508404
878.199347	169.031589	49.513409
874.095220	180.649009	49.518413
871.153886	185.400705	49.523418
867.103506	186.034763	49.528423
863.811950	169.462575	49.533428
860.292368	174.141550	49.538433
856.727209	187.742431	49.543437
853.173392	172.701570	49.548442
850.123915	171.884885	49.553447
846.208439	169.637360	49.558452
842.923246	183.691306	49.563457
839.057387	177.905416	49.568461
835.803188	174.112282	49.573466
832.217823	180.208856	49.578471
829.243924	178.821707	49.583476
825.558793	173.743134	49.588481
822.030041	177.892483	49.593485
818.511155	173.625030	49.598490
814.656955	182.545415	49.603495
811.139099	175.815661	49.608500
807.782244	181.400672	49.613505
804.386035	198.211444	49.618509
800.932048	177.404309	49.623514
797.008548	180.461438	49.628519
793.477002	174.937744	49.633524
790.200675	175.439090	49.638529
786.668817	176.697589	49.643533
783.516790	160.710237	49.648538
780.029787	174.014499	49.653543
776.351551	181.727311	49.658548
773.056084	168.843162	49.663553
769.187300	179.208805	49.668557
765.977286	170.957888	49.673562
761.761068	175.744062	49.678567
758.818224	181.288249	49.683572
755.309680	176.914943	49.688577
751.605801	167.593601	49.693581
748.217014	169.660153	49.698586
744.270376	171.830376	49.703591
741.449138	177.057929	49.708596
737.937875	162.723307	49.713601
734.193154	178.275679	49.718605
730.747355	170.758943	49.723610
727.168974	173.849186	49.728615
723.726290	164.230199	49.733620
720.708651	171.866198	49.738625
716.573258	175.577424	49.743629
713.105311	169.561446	49.748634
709.802605	168.165418	49.753639
706.007696	170.465986	49.758644
702.701832	165.872783	49.763649
699.111229	174.385947	49.768653
695.610213	167.961485	49.773658
691.974616	160.609998	49.778663
688.643182	162.261339	49.783668
685.524057	159.762530	49.788673
681.543322	171.922386	49.793677
678.398554	166.904321	49.798682
674.435743	170.605615	49.803687
671.450124	177.226515	49.808692
668.179666	166.191932	49.813697
664.128619	173.797765	49.818701
660.562739	168.833769	49.823706
657.014418	165.295202	49.828711
653.592262	171.594868	49.833716
650.001919	161.342683	49.838721
646.599678	170.566445	49.843725
643.252449	164.728079	49.848730
639.566218	166.595299	49.853735
635.863461	168.594093	49.858740
632.930603	162.690453	49.863745
629.185525	162.122831	49.868749
625.465414	162.995196	49.873754
621.777658	167.260974	49.878759
618.702859	155.717315	49.883764
615.395092	163.569671	49.888769
611.611416	172.325784	49.893773
608.655465	168.824266	49.898778
604.409024	159.852003	49.903783
601.121074	165.676994	49.908788
597.943059	161.259354	49.913793
594.259881	160.432623	49.918797
590.542485	158.959833	49.923802
586.951406	166.065615	49.928807
583.415233	170.929382	49.933812
580.197957	158.002262	49.938817
576.274578	164.835007	49.943821
572.911184	153.458514	49.948826
569.420267	154.975843	49.953831
565.965812	160.530709	49.958836
562.615584	160.140006	49.963841
558.839301	166.004142	49.968845
556.024223	158.727843	49.973850
552.678705	152.132768	49.978855
548.566255	152.120528	49.983860
545.295145	150.862221	49.988865
541.778914	163.511493	49.993869
538.474950	158.669065	49.998874
534.574550	151.029153	50.003879
530.784870	155.184053	50.008884
527.363242	160.424628	50.013889
523.607192	162.122510	50.018893
520.384923	157.479397	50.023898
516.637962	155.416252	50.028903
513.362895	156.895687	50.033908
509.793772	145.009341	50.038913
506.458725	165.900884	50.043917
503.173754	163.920070	50.048922
499.910053	150.327260	50.053927
495.802673	161.035500	50.058932
492.602058	153.701081	50.063937
488.829844	165.640913	50.068941
485.200793	163.888900	50.073946
482.020174	158.772489	50.078951
478.269295	161.336124	50.083956
474.812444	160.119780	50.088961
471.243206	170.608724	50.093965
468.332594	162.934688	50.098970
464.614248	153.998321	50.103975
461.036852	160.015813	50.108980
457.567177	167.211010	50.113985
453.806043	166.079076	50.118989
450.498008	143.981712	50.123994
447.214103	163.148036	50.128999
443.375008	174.067904	50.134004
440.049530	161.714564	50.139009
436.128943	168.945981	50.144013
432.935134	161.784889	50.149018
429.797269	167.699208	50.154023
426.051872	165.431248	50.159028
422.458932	149.254559	50.164033
419.033855	151.897885	50.169037
415.426722	158.089799	50.174042
411.884472	154.854230	50.179047
408.048423	160.420908	50.184052
405.053866	153.851206	50.189057
401.015640	156.590208	50.194061
398.016262	157.190526	50.199066
394.496923	153.267211	50.204071
390.727792	155.915891	50.209076
387.232041	150.441783	50.214081
383.666720	170.222676	50.219085
380.491889	157.885235	50.224090
376.997228	155.720809	50.229095
373.350545	160.848088	50.234100
369.986318	155.266037	50.239105
366.205579	163.337316	50.244109
363.061295	166.556103	50.249114
359.365815	163.889660	50.254119
355.786427	151.552088	50.259124
352.682171	159.760618	50.264129
349.038950	157.377467	50.269133
345.410215	148.218219	50.274138
341.833662	159.573719	50.279143
338.114479	155.552439	50.284148
335.180389	147.294578	50.289153
331.404394	156.059614	50.294157
327.872490	165.225413	50.299162
324.389210	151.116233	50.304167
320.439453	159.273662	50.309172
317.367100	155.178385	50.314177
313.786318	158.768426	50.319181
310.608857	154.771415	50.324186
307.045812	151.555720	50.329191
303.139386	156.633113	50.334196
300.101672	154.005526	50.339201
295.936534	158.366422	50.344205
292.828958	156.583812	50.349210
289.684557	145.834185	50.354215
285.631215	151.710888	50.359220
282.339605	152.058842	50.364225
278.623795	163.608446	50.369229
275.528403	160.009281	50.374234
271.727303	155.157490	50.379239
268.188557	169.179723	50.384244
264.988598	160.683963	50.389249
261.057596	147.931406	50.394253
257.357605	146.454755	50.399258
254.265527	150.901101	50.404263
250.663245	144.234882	50.409268
247.404793	143.221768	50.414273
243.700132	161.111137	50.419277
240.285830	152.486453	50.424282
237.039498	148.455284	50.429287
232.991441	157.006943	50.434292
229.999903	149.518170	50.439297
226.463444	160.254256	50.444301
222.731220	155.607170	50.449306
218.970114	161.072088	50.454311
215.478519	152.350190	50.459316
212.686130	154.872609	50.464321
208.680645	160.926526	50.469325
205.398349	145.076028	50.474330
201.513180	155.372817	50.479335
198.138775	154.145766	50.484340
194.894283	143.093788	50.489345
191.445487	148.522109	50.494349
187.390351	154.386340	50.499354
183.940270	153.509001	50.504359
180.618465	156.318388	50.509364
177.540760	150.042825	50.514369
173.539479	154.332030	50.519373
170.268693	147.186775	50.524378
166.758939	152.285417	50.529383
162.830956	150.057655	50.534388
159.741757	145.684083	50.539393
156.061459	157.200149	50.544397
152.700059	154.425359	50.549402
149.237769	148.148248	50.554407
145.623459	153.135631	50.559412
142.434419	141.647451	50.564417
138.765851	155.472656	50.569421
135.294158	157.471231	50.574426
131.634552	158.109243	50.579431
128.062232	157.785063	50.584436
124.779598	152.156527	50.589441
121.063866	155.315061	50.594445
117.622780	150.354260	50.599450
114.366745	142.796597	50.604455
110.536569	153.992651	50.609460
106.891386	141.258001	50.614465
103.356463	141.196390	50.619469
99.977493	148.382282	50.624474
96.997087	140.991782	50.629479
93.215911	151.303107	50.634484
89.516495	145.655761	50.639489
85.943856	155.788203	50.644493
82.486925	154.638682	50.649498
79.161906	148.352742	50.654503
75.470397	151.815789	50.659508
72.205325	149.097144	50.664513
68.742981	151.135545	50.669517
65.235242	145.784763	50.674522
61.424331	153.605368	50.679527
57.679880	148.322217	50.684532
54.803534	137.887840	50.689537
51.124244	149.060762	50.694541
47.458616	136.296390	50.699546
44.249506	142.175877	50.704551
40.066545	159.781810	50.709556
36.611014	146.892449	50.714561
33.574397	142.255630	50.719565
30.406628	137.372840	50.724570
26.863597	146.567341	50.729575
23.233297	147.253549	50.734580
19.692472	140.861250	50.739585
16.152046	149.961606	50.744589
12.560527	147.067375	50.749594
9.158143	148.974554	50.754599
5.390348	155.707900	50.759604
2.148277	140.959474	50.764609