Thu Jun 16 11:47:12 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
0.115996	86.135293	0.000000
0.551087	93.525130	0.005005
0.748728	98.505532	0.010010
0.870380	104.180289	0.015014
0.561258	84.207745	0.020019
0.582973	82.747916	0.025024
-0.050050	94.494714	0.030029
-0.078030	67.953843	0.035034
-0.553247	57.977415	0.040038
-0.815857	67.591357	0.045043
-0.558950	54.377478	0.050048
-0.838751	44.006806	0.055053
-1.081507	40.163720	0.060058
-1.499687	29.759989	0.065062
-1.772457	24.722837	0.070067
-1.695407	21.573707	0.075072
-2.734016	22.600952	0.080077
-3.023684	8.965827	0.085082
-3.273225	9.653622	0.090086
-3.250921	9.856893	0.095091
-3.425691	-3.331765	0.100096
-4.240343	12.883482	0.105101
-4.030916	2.555501	0.110106
-4.753057	-2.801299	0.115110
-4.527324	17.464658	0.120115
-4.745638	0.249270	0.125120
-5.556915	12.318859	0.130125
-5.900223	11.558238	0.135130
-6.138754	7.397392	0.140134
-6.535868	9.208570	0.145139
-6.376132	10.233796	0.150144
-6.571733	14.868663	0.155149
-6.511988	0.537022	0.160154
-6.282590	3.736786	0.165158
-6.872460	8.316650	0.170163
-7.589617	1.501428	0.175168
-7.668105	9.935992	0.180173
-7.759842	-0.231922	0.185178
-7.957229	1.036409	0.190182
-9.232341	3.732979	0.195187
-9.019878	-2.255559	0.200192
-9.548951	15.385679	0.205197
-9.399223	5.040334	0.210202
-9.619481	9.640405	0.215206
-9.547478	7.101789	0.220211
-9.337660	8.956400	0.225216
-9.815276	12.563937	0.230221
-10.504299	-0.100433	0.235226
-10.730419	12.744050	0.240230
-11.146425	14.427043	0.245235
-10.868120	0.733675	0.250240
-11.605006	6.895171	0.255245
-12.366969	4.068494	0.260250
-12.752705	4.963279	0.265254
-12.862717	11.300956	0.270259
-12.120063	4.609988	0.275264
-12.587012	0.377586	0.280269
-12.756672	-0.719430	0.285274
-12.731379	0.387403	0.290278
-13.693425	1.541392	0.295283
-13.944526	6.214531	0.300288
-14.596186	21.670056	0.305293
-14.336014	10.509930	0.310298
-14.699542	10.685909	0.315302
-14.758360	20.008262	0.320307
-14.394402	8.859299	0.325312
-15.334962	14.231495	0.330317
-15.623062	15.195578	0.335322
-16.234949	23.456871	0.340326
-15.907985	12.418295	0.345331
-15.628014	16.006485	0.350336
-16.270961	16.030645	0.355341
-16.545940	14.056843	0.360346
-17.397056	12.739296	0.365350
-17.572286	18.810540	0.370355
-17.334943	8.671893	0.375360
-17.473479	2.936299	0.380365
-17.830680	23.900778	0.385370
-18.347312	11.545895	0.390374
-18.725988	18.704276	0.395379
-18.700164	14.849564	0.400384
-18.955120	19.301967	0.405389
-18.892798	15.763325	0.410394
-19.637199	6.514494	0.415398
-20.589203	13.929021	0.420403
-20.471855	13.315522	0.425408
-20.766598	12.849938	0.430413
-20.664533	7.585307	0.435418
-20.731180	24.298164	0.440422
-21.092193	18.766253	0.445427
-20.747370	14.215801	0.450432
-20.879631	13.040094	0.455437
-21.789402	15.924599	0.460442
-22.185204	11.967320	0.465446
-22.484039	-0.192008	0.470451
-22.255942	9.742711	0.475456
-22.588730	7.475698	0.480461
-23.499834	5.682299	0.485466
-23.708780	12.028139	0.490470
-23.832351	17.186295	0.495475
-24.101698	8.935061	0.500480
-24.066511	12.628322	0.505485
-23.688995	10.632020	0.510490
-24.148220	11.365124	0.515494
-24.548518	16.465230	0.520499
-24.657653	12.217592	0.525504
-25.347343	15.038005	0.530509
-25.614414	7.178344	0.535514
-25.663665	16.072241	0.540518
-26.542454	9.769498	0.545523
-26.637565	8.883709	0.550528
-27.222472	17.877479	0.555533
-27.246002	15.606905	0.560538
-26.801826	8.165089	0.565542
-27.285539	12.455721	0.570547
-26.938577	5.283905	0.575552
-27.115484	7.198087	0.580557
-28.208684	9.674000	0.585562
-28.366008	12.922878	0.590566
-28.785805	21.692944	0.595571
-28.515574	1.014402	0.600576
-29.138259	4.291749	0.605581
-29.259486	10.379517	0.610586
-29.903778	8.045898	0.615590
-30.338625	13.738008	0.620595
-29.949419	9.988288	0.625600
-30.312598	7.130730	0.630605
-30.534702	12.650158	0.635610
-30.483616	6.313603	0.640614
-31.081017	10.925297	0.645619
-31.426751	-11.010473	0.650624
-31.860048	7.358668	0.655629
-32.159578	10.662716	0.660634
-32.142280	4.381369	0.665638
-32.312383	16.130524	0.670643
-32.227718	13.888437	0.675648
-32.583729	10.724067	0.680653
-33.264913	12.211752	0.685658
-33.554843	10.560255	0.690662
-33.279673	10.832128	0.695667
-33.277224	6.914789	0.700672
-33.783016	11.447613	0.705677
-34.452776	-0.211110	0.710682
-34.570104	8.922020	0.715686
-35.142594	7.132346	0.720691
-34.891774	0.507372	0.725696
-35.273735	17.812752	0.730701
-35.533590	13.425075	0.735706
-36.345533	3.394835	0.740710
-36.591271	7.663499	0.745715
-36.645439	15.703577	0.750720
-36.659731	12.542811	0.755725
-36.955382	13.816137	0.760730
-36.734192	10.534079	0.765734
-36.832021	8.982931	0.770739
-37.261117	4.708266	0.775744
-38.059320	13.182459	0.780749
-38.010122	14.178599	0.785754
-38.407288	15.222070	0.790758
-38.285341	16.889556	0.795763
-38.511325	1.459089	0.800768
-39.484801	11.524122	0.805773
-39.883476	2.075607	0.810778
-40.061260	2.783211	0.815782
-40.325220	1.751206	0.820787
-40.415898	2.789799	0.825792
-40.392668	9.572476	0.830797
-40.472532	11.485518	0.835802
-40.509736	14.597345	0.840806
-40.711434	11.909912	0.845811
-40.937308	-0.806529	0.850816
-41.571670	9.687140	0.855821
-41.721205	4.668106	0.860826
-42.176499	14.539476	0.865830
-42.262215	2.948585	0.870835
-42.840298	1.043623	0.875840
-43.326794	21.444056	0.880845
-43.381950	4.139556	0.885850
-43.158703	6.036833	0.890854
-43.483632	20.049619	0.895859
-43.692689	3.589375	0.900864
-43.537362	4.532460	0.905869
-44.279340	9.035359	0.910874
-44.567192	15.449485	0.915878
-44.763693	15.441990	0.920883
-44.768102	-0.453938	0.925888
-45.587995	10.896809	0.930893
-46.195546	10.194364	0.935898
-46.070365	0.562495	0.940902
-46.602721	4.814403	0.945907
-46.270122	6.882725	0.950912
-46.779286	13.387094	0.955917
-46.215658	18.543845	0.960922
-46.576361	12.306125	0.965926
-47.277632	7.564138	0.970931
-47.741475	6.762079	0.975936
-48.116804	8.948979	0.980941
-48.087716	8.452469	0.985946
-48.490032	11.263172	0.990950
-48.379468	16.744589	0.995955
-49.037179	13.762770	1.000960
-49.320444	13.238861	1.005965
-49.730367	13.518993	1.010970
-50.097049	-5.378160	1.015974
-50.033550	6.539451	1.020979
-49.718300	13.472358	1.025984
-49.929031	5.952818	1.030989
-50.209653	4.623662	1.035994
-50.615430	11.726637	1.040998
-51.314963	9.808699	1.046003
-50.872834	-3.254807	1.051008
-51.283549	4.940377	1.056013
-52.091873	-0.870181	1.061018
-52.730178	3.836467	1.066022
-52.880915	3.211141	1.071027
-52.964645	3.319768	1.076032
-52.909298	9.371841	1.081037
-52.789334	-1.309719	1.086042
-52.932762	8.081162	1.091046
-53.525237	12.058493	1.096051
-53.817830	0.116556	1.101056
-54.216537	3.550148	1.106061
-54.167488	7.960197	1.111066
-54.282352	-4.195887	1.116070
-54.609937	2.368341	1.121075
-55.082184	4.105517	1.126080
-56.143719	8.728907	1.131085
-56.272883	2.902289	1.136090
-55.542483	6.502845	1.141094
-55.869762	9.091707	1.146099
-55.691568	7.325356	1.151104
-56.602251	14.432264	1.156109
-57.171132	13.998277	1.161114
-57.095842	2.294654	1.166118
-57.330104	13.505504	1.171123
-57.445798	6.445963	1.176128
-57.698544	6.039044	1.181133
-58.624228	6.172878	1.186138
-58.590256	8.178682	1.191142
-58.769185	10.012106	1.196147
-59.065572	4.150974	1.201152
-59.273061	19.538709	1.206157
-59.350780	7.988323	1.211162
-59.397848	-3.026896	1.216166
-60.055366	9.420768	1.221171
-60.317921	9.183378	1.226176
-60.996309	5.964859	1.231181
-60.838022	5.912144	1.236186
-60.838355	4.613022	1.241190
-61.179700	2.646542	1.246195
-60.990432	2.307645	1.251200
-61.523248	10.203475	1.256205
-61.693577	10.513757	1.261210
-61.946194	2.252663	1.266214
-62.514379	7.820901	1.271219
-62.061527	-0.762773	1.276224
-62.909324	5.060820	1.281229
-63.433274	16.788249	1.286234
-63.775147	-0.028765	1.291238
-64.234367	1.501061	1.296243
-64.137691	10.754791	1.301248
-64.350505	4.182667	1.306253
-64.825295	-3.607730	1.311258
-64.506658	-2.168382	1.316262
-64.205750	16.547728	1.321267
-64.238853	8.019800	1.326272
-65.617293	19.967476	1.331277
-65.918496	10.876844	1.336282
-66.019942	4.286117	1.341286
-66.163019	12.202869	1.346291
-66.149401	16.927066	1.351296
-66.883370	12.321299	1.356301
-67.617476	2.176589	1.361306
-67.792268	6.063973	1.366310
-67.346884	12.928805	1.371315
-67.696245	-1.477370	1.376320
-67.633648	11.475852	1.381325
-67.995360	11.630916	1.386330
-67.575314	11.191627	1.391334
-68.409977	18.246315	1.396339
-68.534276	10.177298	1.401344
-68.833137	10.007962	1.406349
-69.730263	9.142261	1.411354
-69.924917	16.286110	1.416358
-70.520649	16.980022	1.421363
-70.250892	-3.715890	1.426368
-70.589090	11.307212	1.431373
-70.802257	9.754805	1.436378
-70.604395	15.870435	1.441382
-70.943880	11.115221	1.446387
-71.315199	5.067294	1.451392
-71.980299	7.664044	1.456397
-72.164626	9.389448	1.461402
-72.046569	8.606839	1.466406
-72.433877	12.409189	1.471411
-72.144004	1.810235	1.476416
-73.208306	12.067067	1.481421
-73.679812	5.409943	1.486426
-73.707573	5.728231	1.491430
-74.307714	5.455283	1.496435
-73.249041	10.334285	1.501440
-74.078673	11.087867	1.506445
-74.191095	12.188061	1.511450
-74.157356	-0.473811	1.516454
-74.909266	0.109278	1.521459
-75.271208	-0.641944	1.526464
-75.436716	6.124372	1.531469
-75.689525	0.741808	1.536474
-75.445852	0.064714	1.541478
-76.516453	10.949130	1.546483
-76.733045	-7.128251	1.551488
-77.017624	8.148697	1.556493
-76.917996	7.165712	1.561498
-76.757595	2.290692	1.566502
-77.164901	14.043332	1.571507
-77.389825	13.384099	1.576512
-78.523168	12.951262	1.581517
-78.882487	11.752412	1.586522
-78.569360	8.718760	1.591526
-79.133327	5.425002	1.596531
-78.793148	14.443253	1.601536
-78.799711	13.637143	1.606541
-79.010629	8.373534	1.611546
-79.622529	2.942096	1.616550
-80.388776	15.380112	1.621555
-80.293871	7.811146	1.626560
-80.474952	14.856071	1.631565
-80.354693	27.343603	1.636570
-80.354405	15.517609	1.641574
-81.341890	12.344455	1.646579
-81.468785	17.809772	1.651584
-81.997642	21.721149	1.656589
-82.256238	5.310731	1.661594
-81.987746	16.858059	1.666598
-82.134950	9.001580	1.671603
-82.338448	12.312742	1.676608
-82.962225	10.196919	1.681613
-83.532535	8.228822	1.686618
-83.315673	10.134946	1.691622
-84.009660	24.301165	1.696627
-83.733550	6.409786	1.701632
-84.215126	5.151136	1.706637
-84.817518	11.540987	1.711642
-85.213391	9.834000	1.716646
-85.476460	13.948179	1.721651
-85.373588	2.610541	1.726656
-85.630225	2.731567	1.731661
-85.655081	13.667585	1.736666
-85.281110	6.930015	1.741670
-86.013192	12.372727	1.746675
-86.207667	15.119288	1.751680
-86.739550	9.260282	1.756685
-87.251035	14.671073	1.761690
-87.147102	17.700578	1.766694
-87.092965	18.858679	1.771699
-86.906810	17.760963	1.776704
-88.189641	22.189397	1.781709
-88.538332	13.863876	1.786714
-88.601654	7.680894	1.791718
-88.638062	7.045947	1.796723
-88.586845	13.267003	1.801728
-89.226624	9.870548	1.806733
-89.955097	14.023764	1.811738
-89.974573	10.419722	1.816742
-90.545026	20.845024	1.821747
-90.199069	11.806068	1.826752
-90.276222	14.439025	1.831757
-90.518151	20.082285	1.836762
-90.559065	-4.395929	1.841766
-91.288033	2.752268	1.846771
-91.606486	-0.579204	1.851776
-91.656065	-0.745050	1.856781
-91.743188	3.895659	1.861786
-91.741325	5.019780	1.866790
-92.671136	-1.091116	1.871795
-93.087912	-2.728943	1.876800
-93.427116	0.147390	1.881805
-93.452572	-2.064557	1.886810
-93.604659	-1.228510	1.891814
-93.814346	3.812466	1.896819
-93.547193	-6.920246	1.901824
-94.018421	-1.132453	1.906829
-94.955149	5.812232	1.911834
-95.383421	-8.110117	1.916838
-95.561335	2.786374	1.921843
-95.360247	-8.490242	1.926848
-95.708896	2.631675	1.931853
-95.562375	-1.047844	1.936858
-95.550602	4.870253	1.941862
-95.847112	6.643301	1.946867
-95.826583	2.808707	1.951872
-96.765297	11.498596	1.956877
-97.082164	-2.526025	1.961882
-96.962538	0.997106	1.966886
-97.529698	4.871502	1.971891
-97.877133	12.563657	1.976896
-98.340148	0.175769	1.981901
-98.947623	1.884295	1.986906
-98.861636	-1.772295	1.991910
-99.113392	1.206982	1.996915
-99.018216	-0.890377	2.006912
-98.067015	4.336138	2.016909
-98.176771	6.113009	2.026906
-97.556514	-1.606550	2.036902
-97.420590	0.920342	2.046899
-97.065462	-0.790616	2.056896
-96.164658	2.118128	2.066893
-95.713987	4.078855	2.076890
-95.004914	2.236548	2.086886
-94.416092	-2.622059	2.096883
-94.077282	-5.191723	2.106880
-94.098226	-3.304577	2.116877
-93.112252	5.899808	2.126874
-92.667832	3.909018	2.136870
-92.253597	0.628222	2.146867
-91.521065	5.172113	2.156864
-91.319148	3.367349	2.166861
-90.949905	4.922069	2.176858
-90.082765	11.220308	2.186854
-89.771875	1.380958	2.196851
-89.132749	5.746977	2.206848
-88.210384	1.004575	2.216845
-88.286175	6.333858	2.226842
-87.857830	6.964065	2.236838
-86.923405	-0.045288	2.246835
-86.956043	9.961122	2.256832
-86.322448	3.207393	2.266829
-85.517306	3.026776	2.276826
-85.425742	6.558030	2.286822
-84.515712	2.300795	2.296819
-83.694220	-2.167021	2.306816
-83.383660	1.629363	2.316813
-83.522358	-5.542476	2.326810
-83.254025	4.968289	2.336806
-82.509120	-5.018750	2.346803
-81.201353	8.442535	2.356800
-80.638123	7.240172	2.366797
-80.663209	-1.236453	2.376794
-80.392551	12.157298	2.386790
-80.048946	17.081617	2.396787
-78.892484	12.198483	2.406784
-78.741624	9.394708	2.416781
-78.290708	6.255771	2.426778
-77.371721	14.078696	2.436774
-77.691243	3.818079	2.446771
-76.656340	14.856026	2.456768
-76.233700	3.699504	2.466765
-75.600427	18.288962	2.476762
-74.662334	5.825200	2.486758
-74.495582	14.459312	2.496755
-74.605164	7.952031	2.506752
-73.534394	9.146676	2.516749
-72.812134	7.620705	2.526746
-73.323746	4.287515	2.536742
-72.378378	11.852514	2.546739
-71.681056	8.445709	2.556736
-70.539664	7.286972	2.566733
-70.803550	5.811377	2.576730
-69.963938	9.503385	2.586726
-69.586107	7.713652	2.596723
-69.273932	7.181907	2.606720
-68.499656	1.738597	2.616717
-68.000893	7.092051	2.626714
-67.652635	8.843947	2.636710
-66.970033	7.932369	2.646707
-66.792105	16.602863	2.656704
-66.228217	2.957022	2.666701
-65.136285	2.244052	2.676698
-64.968210	7.289492	2.686694
-64.923928	14.647418	2.696691
-64.341494	13.225358	2.706688
-63.758179	9.191182	2.716685
-63.230698	5.289808	2.726682
-62.222647	11.073485	2.736678
-61.968745	10.226487	2.746675
-61.877991	5.405992	2.756672
-61.358507	7.868853	2.766669
-60.369062	7.305730	2.776666
-60.319023	1.143975	2.786662
-59.363951	-3.964126	2.796659
-58.477668	5.252101	2.806656
-58.602509	-3.428810	2.816653
-58.554205	2.957398	2.826650
-57.748166	-0.302904	2.836646
-57.158951	3.395174	2.846643
-56.483168	-4.398062	2.856640
-55.649365	0.843862	2.866637
-55.471792	-1.127073	2.876634
-55.213189	2.435841	2.886630
-55.153831	10.953956	2.896627
-53.792886	2.080084	2.906624
-53.547194	6.651497	2.916621
-53.186365	-4.839939	2.926618
-52.616594	-10.053814	2.936614
-52.471159	0.195546	2.946611
-51.314196	-6.440893	2.956608
-50.763628	-8.149033	2.966605
-50.947012	-2.692473	2.976602
-50.136369	0.244564	2.986598
-49.615563	-2.120528	2.996595
-49.141234	-0.938383	3.006592
-48.409419	-1.426971	3.016589
-47.781278	3.500898	3.026586
-47.635017	0.024753	3.036582
-47.581159	9.841834	3.046579
-46.636032	-6.328785	3.056576
-46.386831	1.261381	3.066573
-44.950387	5.455529	3.076570
-44.622049	7.702541	3.086566
-44.521532	19.141875	3.096563
-44.357758	10.895594	3.106560
-43.772064	11.680369	3.116557
-43.332189	7.170867	3.126554
-42.228535	9.399438	3.136550
-41.668473	9.032139	3.146547
-41.411342	6.858051	3.156544
-41.103518	2.756553	3.166541
-41.029345	12.516593	3.176538
-40.258860	7.569830	3.186534
-39.565455	1.337602	3.196531
-38.927697	4.862452	3.206528
-38.238279	3.078814	3.216525
-37.965522	6.038666	3.226522
-37.934712	9.500249	3.236518
-36.936041	6.044137	3.246515
-36.638840	9.090531	3.256512
-36.104247	2.219172	3.266509
-35.110807	11.025544	3.276506
-34.841222	10.477627	3.286502
-34.703226	9.942765	3.296499
-34.172284	-8.347906	3.306496
-33.391487	2.810126	3.316493
-33.279387	-4.569116	3.326490
-32.581953	4.256589	3.336486
-31.730731	8.566425	3.346483
-31.571546	10.811958	3.356480
-31.093225	4.740330	3.366477
-30.250497	13.930478	3.376474
-30.242702	9.703378	3.386470
-29.807643	3.903233	3.396467
-28.907881	3.491449	3.406464
-28.197626	6.362008	3.416461
-28.214519	3.698664	3.426458
-27.347519	0.455405	3.436454
-27.008439	-1.681106	3.446451
-26.733215	-5.953239	3.456448
-26.222977	9.721939	3.466445
-25.667741	3.625599	3.476442
-24.809509	1.526467	3.486438
-24.118951	0.023669	3.496435
-24.157825	12.102369	3.506432
-23.816405	0.987915	3.516429
-22.831117	5.133453	3.526426
-22.277470	17.462678	3.536422
-22.096061	18.372796	3.546419
-21.606415	7.024232	3.556416
-20.861836	11.379008	3.566413
-20.842681	5.941466	3.576410
-20.251873	19.903597	3.586406
-19.245751	5.955644	3.596403
-19.045161	2.130669	3.606400
-18.346032	3.996704	3.616397
-17.523550	1.393435	3.626394
-17.345985	12.295367	3.636390
-17.251363	6.769292	3.646387
-16.653867	7.736145	3.656384
-15.684901	7.551774	3.666381
-15.363853	9.407099	3.676378
-15.404802	8.624882	3.686374
-14.380658	15.740816	3.696371
-14.117460	3.476902	3.706368
-13.428495	7.652744	3.716365
-12.658846	13.123191	3.726362
-12.186851	8.716495	3.736358
-12.310688	11.581673	3.746355
-11.748426	13.471367	3.756352
-10.953699	11.041448	3.766349
-10.594485	7.251895	3.776346
-9.600757	15.049890	3.786342
-9.307493	12.290935	3.796339
-8.874344	10.745727	3.806336
-8.848550	12.853284	3.816333
-7.693815	7.159221	3.826330
-7.526585	10.051170	3.836326
-7.376114	8.570855	3.846323
-6.219822	7.893981	3.856320
-5.857122	2.998958	3.866317
-5.918375	5.772250	3.876314
-5.058693	8.668199	3.886310
-4.653736	7.924503	3.896307
-3.760738	16.044523	3.906304
-3.377053	23.210547	3.916301
-3.451628	24.401375	3.926298
-3.240406	41.303360	3.936294
-2.579183	58.773607	3.946291
-1.485724	70.449637	3.956288
-0.773475	85.194150	3.966285
-0.907440	83.228214	3.976282
-0.496132	107.445634	3.986278
0.000000	110.834387	3.991283
0.036228	116.792590	3.996288
0.541534	124.882231	4.001293
0.464163	145.365174	4.006298
0.639910	126.617241	4.011302
0.503792	123.268919	4.016307
0.295063	134.037520	4.021312
0.606042	127.765101	4.026317
0.850781	149.292143	4.031322
1.068621	137.413913	4.036326
0.558742	141.591900	4.041331
0.439424	147.952284	4.046336
0.869219	152.178011	4.051341
0.652325	166.366146	4.056346
1.035632	157.595779	4.061350
1.250920	157.256527	4.066355
1.154482	160.915048	4.071360
1.078780	149.779449	4.076365
0.736292	154.470400	4.081370
0.878214	142.537627	4.086374
0.851592	156.136321	4.091379
1.049340	170.223872	4.096384
1.371361	162.887209	4.101389
1.163398	152.673880	4.106394
0.873016	145.225340	4.111398
0.729823	145.564286	4.116403
0.766025	152.201344	4.121408
1.317495	148.848495	4.126413
1.157363	165.581102	4.131418
1.018501	160.955655	4.136422
1.185233	170.251776	4.141427
1.114253	166.027385	4.146432
1.071055	158.707278	4.151437
1.115459	171.138615	4.156442
1.232690	172.324284	4.161446
1.040461	165.442459	4.166451
1.318244	172.708082	4.171456
1.450452	169.741196	4.176461
1.035638	157.746716	4.181466
1.184861	147.859506	4.186470
1.212780	153.940145	4.191475
1.072862	152.193696	4.196480
1.297237	158.863686	4.201485
1.112874	164.679306	4.206490
1.312653	159.708543	4.211494
1.073910	166.402687	4.216499
1.328740	169.764713	4.221504
1.304162	168.118572	4.226509
1.063441	174.292251	4.231514
1.300649	169.511720	4.236518
1.204809	171.306274	4.241523
1.237908	175.293219	4.246528
1.420559	168.461905	4.251533
1.318412	168.624087	4.256538
1.486284	164.685288	4.261542
1.210856	164.947630	4.266547
0.837843	170.175375	4.271552
1.287160	170.396079	4.276557
1.070382	181.850506	4.281562
1.166250	161.379616	4.286566
1.318300	167.669019	4.291571
1.118305	168.717795	4.296576
1.475834	176.629349	4.301581
1.999872	197.261580	4.306586
1.709803	186.780140	4.311590
1.311489	168.645059	4.316595
1.545029	180.929327	4.321600
1.572478	168.543590	4.326605
1.614533	167.590728	4.331610
1.492337	173.835483	4.336614
1.742727	179.131766	4.341619
1.693562	175.098115	4.346624
1.718405	174.651825	4.351629
1.656688	170.137832	4.356634
1.491195	165.263244	4.361638
1.469848	172.147578	4.366643
1.699775	194.702049	4.371648
1.681888	168.532051	4.376653
1.463711	172.834583	4.381658
1.795471	185.266980	4.386662
2.023311	191.485168	4.391667
1.640913	189.191499	4.396672
1.532112	167.468468	4.401677
1.849945	184.060349	4.406682
2.057752	186.106112	4.411686
1.745354	176.849609	4.416691
1.786542	173.695819	4.421696
2.166659	164.966325	4.426701
1.695448	173.206915	4.431706
1.771248	166.839078	4.436710
1.842730	165.415312	4.441715
1.549247	179.287302	4.446720
1.751481	176.031131	4.451725
2.054332	183.356643	4.456730
1.986696	180.456619	4.461734
1.806840	181.680337	4.466739
1.801820	169.581129	4.471744
1.648427	184.413059	4.476749
1.694066	201.048166	4.481754
1.888959	197.406873	4.486758
1.796482	201.776737	4.491763
1.576919	207.220345	4.496768
1.783437	199.711264	4.501773
1.931640	195.846245	4.506778
2.048348	189.831924	4.511782
1.922545	198.664096	4.516787
1.785956	202.421998	4.521792
2.229208	197.770580	4.526797
2.074324	193.123601	4.531802
2.049733	194.374045	4.536806
1.959209	200.260691	4.541811
1.994465	195.544700	4.546816
2.409627	189.660902	4.551821
1.954283	187.604714	4.556826
2.158665	193.242549	4.561830
1.948085	194.345265	4.566835
2.136917	198.928198	4.571840
2.309491	194.579889	4.576845
2.193692	196.885617	4.581850
1.991869	201.343004	4.586854
2.030094	192.129963	4.591859
1.903781	194.382774	4.596864
2.677781	205.823928	4.601869
2.354548	216.179009	4.606874
2.095310	196.703580	4.611878
2.296189	205.730377	4.616883
1.919570	207.787884	4.621888
2.500185	203.755411	4.626893
2.533185	218.762561	4.631898
1.958150	210.729051	4.636902
2.629664	220.176776	4.641907
2.598089	201.957864	4.646912
2.374357	199.013194	4.651917
2.145551	197.361340	4.656922
2.205260	194.595846	4.661926
2.245857	196.492752	4.666931
2.185356	223.062641	4.671936
2.564668	220.030640	4.676941
2.563554	230.781275	4.681946
2.213513	233.485414	4.686950
2.505755	225.238820	4.691955
2.275441	226.831757	4.696960
2.366361	219.931922	4.701965
2.216733	231.297548	4.706970
2.395739	227.752497	4.711974
2.266529	229.279300	4.716979
2.304427	236.545333	4.721984
2.742297	232.058758	4.726989
2.412873	230.056238	4.731994
2.352038	247.220908	4.736998
2.949671	231.471874	4.742003
2.550318	231.849209	4.747008
2.532330	221.175982	4.752013
2.457848	235.363237	4.757018
2.418560	230.430579	4.762022
2.827670	231.478832	4.767027
2.428557	237.247199	4.772032
2.931611	224.144621	4.777037
2.631106	226.596304	4.782042
2.624849	233.312629	4.787046
2.956326	238.504573	4.792051
2.457612	242.380141	4.797056
2.692752	225.070718	4.802061
2.821872	228.062959	4.807066
2.580548	238.025883	4.812070
2.871525	241.606488	4.817075
2.410189	233.283567	4.822080
3.055558	251.338894	4.827085
2.903309	244.297315	4.832090
3.031670	231.496384	4.837094
3.150257	225.514689	4.842099
2.783686	237.278431	4.847104
2.923504	224.060672	4.852109
2.859157	235.359132	4.857114
2.762013	237.530079	4.862118
2.632992	234.613257	4.867123
2.601184	229.855264	4.872128
3.183552	238.835214	4.877133
2.981913	250.683682	4.882138
2.883921	236.877178	4.887142
2.592013	250.277305	4.892147
2.747260	262.592533	4.897152
3.080042	256.538925	4.902157
3.119486	258.584800	4.907162
2.915688	253.565375	4.912166
3.037412	259.452087	4.917171
3.146313	258.556442	4.922176
3.421654	252.582768	4.927181
2.881744	264.530953	4.932186
3.135762	259.857417	4.937190
2.947485	262.969796	4.942195
2.809780	265.539208	4.947200
3.008974	264.973142	4.952205
3.034877	271.231937	4.957210
2.956781	258.607363	4.962214
3.402483	252.167607	4.967219
3.248739	265.291963	4.972224
3.490393	260.492121	4.977229
3.344234	269.156828	4.982234
3.157544	260.273625	4.987238
3.397765	259.242331	4.992243
3.317815	268.607593	4.997248
3.278567	250.825944	5.002253
3.180519	262.677230	5.007258
3.028943	263.885922	5.012262
3.118360	254.470231	5.017267
3.151879	267.090987	5.022272
3.393726	261.359024	5.027277
2.985316	252.761373	5.032282
2.911609	254.904673	5.037286
3.316396	250.676906	5.042291
3.315062	247.058263	5.047296
3.624575	251.646425	5.052301
3.352942	261.496876	5.057306
3.191047	264.914670	5.062310
3.317597	262.849615	5.067315
3.417183	262.320630	5.072320
3.460791	254.221756	5.077325
3.055823	270.776814	5.082330
3.159055	259.609295	5.087334
3.292755	260.137479	5.092339
3.315405	270.047130	5.097344
3.700111	271.632550	5.102349
3.523408	272.871045	5.107354
3.589634	276.855106	5.112358
3.544848	266.186277	5.117363
3.195016	263.456193	5.122368
3.598017	277.920523	5.127373
3.518568	293.557200	5.132378
3.734642	286.917226	5.137382
3.418632	293.357727	5.142387
3.537549	290.073077	5.147392
3.832059	284.787102	5.152397
3.458080	299.141409	5.157402
3.505571	297.945739	5.162406
3.651920	278.030954	5.167411
3.491308	295.807253	5.172416
3.808423	286.001222	5.177421
3.784210	289.555399	5.182426
3.467814	284.432240	5.187430
3.690470	290.516661	5.192435
3.628570	288.834944	5.197440
3.892449	283.927637	5.202445
3.897853	286.082236	5.207450
3.656143	280.323336	5.212454
3.867849	279.982108	5.217459
3.320999	296.689189	5.222464
3.656671	281.462563	5.227469
3.704527	293.779877	5.232474
3.537517	288.963016	5.237478
3.768014	292.755674	5.242483
3.538174	288.833538	5.247488
3.614602	285.031166	5.252493
3.660958	284.276770	5.257498
3.735521	298.965874	5.262502
3.928386	299.678730	5.267507
3.673034	305.959454	5.272512
4.282451	311.682029	5.277517
3.595918	313.699511	5.282522
3.787449	314.517162	5.287526
4.102193	323.647741	5.292531
3.911652	323.794245	5.297536
4.163757	305.079054	5.302541
3.677349	316.835925	5.307546
3.845292	316.950711	5.312550
4.022989	317.949510	5.317555
4.104961	321.412253	5.322560
4.497140	315.833498	5.327565
4.341420	336.105894	5.332570
4.508116	320.207493	5.337574
4.228952	296.073584	5.342579
3.780527	297.911624	5.347584
3.723362	302.483152	5.352589
4.094129	319.116943	5.357594
3.832027	317.721457	5.362598
4.401350	317.382195	5.367603
3.828548	329.612988	5.372608
4.251859	327.691555	5.377613
3.913385	326.609785	5.382618
4.080046	322.271987	5.387622
4.162886	326.018714	5.392627
4.312125	330.177699	5.397632
4.464987	316.059945	5.402637
4.281976	322.378640	5.407642
3.974079	322.599983	5.412646
4.413518	314.143642	5.417651
4.130096	324.593141	5.422656
4.098942	320.442036	5.427661
3.910742	319.279297	5.432666
3.867748	322.518127	5.437670
4.225693	321.497957	5.442675
4.337791	336.535559	5.447680
4.612413	344.763378	5.452685
4.500777	324.774753	5.457690
4.275396	321.445578	5.462694
4.192173	328.736900	5.467699
4.160692	346.178588	5.472704
4.477099	349.274665	5.477709
4.479796	352.653932	5.482714
4.478310	369.724582	5.487718
4.124797	349.869817	5.492723
4.457808	356.898705	5.497728
4.671062	355.492039	5.502733
4.679708	360.726326	5.507738
4.666882	343.190789	5.512742
4.568563	353.854283	5.517747
4.483547	368.016271	5.522752
4.745327	343.594199	5.527757
4.266783	355.260813	5.532762
4.416014	361.349997	5.537766
4.627868	346.080827	5.542771
4.572579	351.644728	5.547776
4.906387	356.828040	5.552781
4.466519	361.681748	5.557786
4.670768	359.534584	5.562790
4.713390	350.691467	5.567795
4.476252	364.857283	5.572800
4.902390	355.777742	5.577805
4.684747	344.561082	5.582810
4.547070	354.118842	5.587814
4.815638	345.944563	5.592819
4.503402	349.540729	5.597824
4.696622	352.914654	5.602829
4.690655	354.396438	5.607834
4.745637	357.196543	5.612838
4.908752	348.962739	5.617843
4.532511	355.231694	5.622848
4.798247	353.585798	5.627853
4.982448	364.232108	5.632858
4.603749	361.759728	5.637862
4.779022	344.694765	5.642867
4.469991	352.385480	5.647872
4.623874	349.828145	5.652877
4.655088	350.277968	5.657882
4.596328	353.110484	5.662886
4.726854	368.040496	5.667891
4.669318	387.877647	5.672896
5.087801	370.897557	5.677901
4.848396	386.898560	5.682906
4.608938	386.677173	5.687910
5.166259	383.108731	5.692915
4.884947	386.522018	5.697920
5.056298	382.432534	5.702925
4.946252	397.756308	5.707930
5.050396	390.003406	5.712934
5.402850	380.681891	5.717939
4.879560	389.496794	5.722944
5.194342	386.104776	5.727949
5.043151	385.130070	5.732954
4.918110	381.296646	5.737958
5.043205	379.520383	5.742963
4.823172	384.391239	5.747968
4.726245	380.158547	5.752973
5.022448	397.563898	5.757978
5.252153	380.503416	5.762982
5.001932	381.562974	5.767987
4.734041	390.855979	5.772992
4.964202	383.971928	5.777997
4.791958	373.658136	5.783002
5.032709	390.688085	5.788006
5.427652	404.901211	5.793011
5.056028	396.182268	5.798016
5.235667	399.035475	5.803021
5.528743	412.549204	5.808026
5.210570	406.279229	5.813030
5.576214	384.964644	5.818035
5.014235	400.610536	5.823040
5.101530	392.493418	5.828045
5.287288	403.976393	5.833050
5.151676	421.273876	5.838054
5.476195	405.368444	5.843059
5.404294	412.765963	5.848064
5.549497	419.205471	5.853069
5.095877	420.917907	5.858074
5.287780	413.500520	5.863078
5.511896	411.302612	5.868083
5.359085	417.255769	5.873088
5.707036	407.086544	5.878093
5.840393	407.178633	5.883098
5.353372	406.113119	5.888102
5.688079	397.148898	5.893107
5.214980	394.488785	5.898112
5.495101	400.139732	5.903117
5.531444	408.803263	5.908122
5.951867	403.591247	5.913126
5.761175	400.128267	5.918131
5.258026	386.735458	5.923136
5.567443	380.606245	5.928141
5.386764	379.234589	5.933146
5.217758	394.062890	5.938150
5.636276	403.884219	5.943155
5.607222	407.100341	5.948160
5.679679	407.397537	5.953165
5.371049	426.308620	5.958170
5.658229	415.189809	5.963174
5.928399	409.066183	5.968179
5.634731	412.977262	5.973184
5.463785	405.810939	5.978189
5.400276	419.672566	5.983194
5.427104	405.350426	5.988198
5.495237	411.562146	5.993203
5.399790	414.675097	5.998208
5.700244	408.698988	6.003213
5.274280	410.385543	6.008218
5.484072	411.668302	6.013222
5.624080	418.307066	6.018227
5.336013	413.412502	6.023232
5.977144	413.930725	6.028237
5.674491	426.979495	6.033242
5.487892	430.422423	6.038246
5.863040	426.038105	6.043251
5.692533	441.860952	6.048256
5.934114	429.823485	6.053261
5.884904	417.546603	6.058266
5.426541	421.008592	6.063270
5.853222	412.390143	6.068275
6.141530	422.580666	6.073280
5.560824	412.252763	6.078285
5.801928	408.610295	6.083290
6.189197	410.157422	6.088294
5.858396	407.993902	6.093299
5.441399	413.355079	6.098304
5.731641	417.736734	6.103309
5.658000	413.385645	6.108314
5.547911	401.282112	6.113318
5.819532	402.229484	6.118323
5.687922	422.094804	6.123328
5.687730	406.514829	6.128333
5.367621	418.521517	6.133338
5.396016	423.243696	6.138342
5.922711	423.565763	6.143347
5.692212	423.512977	6.148352
5.996442	413.096047	6.153357
5.677308	403.164926	6.158362
5.899943	415.358744	6.163366
5.807725	417.734896	6.168371
5.686614	417.535780	6.173376
5.271164	417.997761	6.178381
5.248379	421.944974	6.183386
6.064585	427.962632	6.188390
6.008256	425.191906	6.193395
5.561477	430.922544	6.198400
5.600289	419.222357	6.203405
6.058147	413.234736	6.208410
6.237634	411.844498	6.213414
6.039065	407.209605	6.218419
5.820461	420.461719	6.223424
6.010398	413.787633	6.228429
5.783650	418.920948	6.233434
5.945857	412.384630	6.238438
6.003890	411.521356	6.243443
5.953727	424.022195	6.248448
5.987474	411.684943	6.253453
5.855996	398.103238	6.258458
5.777991	389.814056	6.263462
5.947809	388.049048	6.268467
5.616961	382.759444	6.273472
5.807074	377.096562	6.278477
6.025258	380.370870	6.283482
5.765491	384.384663	6.288486
6.046911	376.879100	6.293491
5.723863	389.822491	6.298496
5.923118	389.488153	6.303501
5.677765	389.565482	6.308506
5.608765	382.977511	6.313510
5.770256	366.974459	6.318515
5.373255	386.155614	6.323520
5.716418	399.544739	6.328525
5.611753	389.132754	6.333530
5.345482	381.902384	6.338534
5.965277	380.541984	6.343539
5.671590	388.638318	6.348544
5.817474	378.700803	6.353549
5.636584	375.411421	6.358554
5.820903	383.642247	6.363558
5.886629	377.197261	6.368563
5.463647	379.799434	6.373568
5.658756	383.828520	6.378573
5.571849	379.437014	6.383578
5.279903	377.863646	6.388582
5.360985	380.437764	6.393587
5.808566	401.208889	6.398592
6.066469	397.048468	6.403597
5.642717	391.227565	6.408602
5.562370	390.962224	6.413606
5.715379	382.696627	6.418611
5.688935	390.909014	6.423616
5.691943	398.292962	6.428621
5.746888	402.746449	6.433626
5.692333	401.763763	6.438630
5.836607	394.266552	6.443635
6.055360	394.440125	6.448640
5.839326	385.258629	6.453645
5.909820	381.178906	6.458650
5.813172	388.989726	6.463654
5.867884	384.205843	6.468659
5.702399	385.707679	6.473664
5.660648	368.521397	6.478669
5.655410	382.963813	6.483674
5.749935	375.080408	6.488678
5.754711	387.458290	6.493683
5.440825	391.313906	6.498688
5.341938	374.705315	6.503693
5.452054	380.600898	6.508698
5.395043	390.372258	6.513702
5.927426	396.460881	6.518707
6.016234	408.109048	6.523712
6.044448	392.326391	6.528717
5.716371	392.747986	6.533722
5.718006	377.916928	6.538726
5.960128	365.699968	6.543731
5.408797	379.276462	6.548736
5.705880	380.006923	6.553741
5.632486	381.673092	6.558746
5.586437	381.229436	6.563750
5.692557	374.639165	6.568755
6.015450	386.772490	6.573760
5.872790	380.542184	6.578765
5.744516	380.647618	6.583770
5.944042	389.812865	6.588774
6.037589	385.969064	6.593779
5.661907	378.601000	6.598784
5.966281	370.203058	6.603789
5.698774	379.550450	6.608794
5.763856	387.187742	6.613798
5.838633	370.224202	6.618803
5.737525	375.841263	6.623808
5.832731	379.713916	6.628813
5.615378	378.603838	6.633818
5.783370	379.285589	6.638822
5.783388	384.806128	6.643827
5.838040	375.958346	6.648832
5.568399	377.990993	6.653837
5.610805	383.221682	6.658842
5.907733	383.548867	6.663846
5.724890	380.020369	6.668851
5.610781	380.400585	6.673856
5.710195	381.733351	6.678861
5.700404	378.780026	6.683866
5.933585	381.068064	6.688870
5.713308	376.396615	6.693875
5.677971	375.386288	6.698880
5.642828	380.475693	6.703885
5.366415	382.859391	6.708890
5.743775	385.352285	6.713894
5.886247	369.716905	6.718899
5.543786	388.097340	6.723904
5.840695	374.067010	6.728909
5.630322	376.446996	6.733914
5.717034	380.721988	6.738918
5.890486	383.039924	6.743923
5.525282	382.813963	6.748928
5.713954	374.859457	6.753933
5.999244	382.908644	6.758938
5.728742	376.974420	6.763942
5.843227	378.488884	6.768947
5.474058	382.352647	6.773952
5.817083	390.195776	6.778957
5.858685	383.857770	6.783962
5.631169	386.958406	6.788966
5.806272	385.178220	6.793971
5.404780	383.990742	6.798976
5.706899	377.410501	6.803981
5.783512	387.714219	6.808986
5.761246	385.121271	6.813990
5.791232	384.235306	6.818995
5.498892	390.611559	6.824000
5.584374	380.125241	6.829005
5.799911	379.098315	6.834010
5.485302	386.607851	6.839014
5.786315	387.136703	6.844019
5.619682	396.770603	6.849024
5.751767	377.052496	6.854029
5.495808	373.699654	6.859034
5.387282	396.309368	6.864038
5.779539	374.953995	6.869043
5.639534	381.323518	6.874048
5.592930	377.564343	6.879053
5.474169	377.642259	6.884058
5.168477	381.551469	6.889062
5.565943	392.899510	6.894067
5.792600	407.311518	6.899072
5.896249	394.554195	6.904077
5.573413	388.635127	6.909082
5.445962	409.550424	6.914086
6.188009	399.741280	6.919091
5.807654	389.543261	6.924096
5.727135	380.587984	6.929101
5.857040	388.147970	6.934106
5.778537	388.605370	6.939110
5.551010	372.542197	6.944115
5.542143	385.131382	6.949120
5.383839	381.827118	6.954125
5.630865	399.899420	6.959130
5.625702	412.630869	6.964134
5.747162	413.167296	6.969139
5.574466	410.248582	6.974144
5.757938	411.132387	6.979149
5.990309	412.729185	6.984154
5.656742	412.839344	6.989158
6.040389	402.930198	6.994163
5.471659	407.065990	6.999168
5.728861	420.909936	7.004173
6.090312	413.303128	7.009178
5.776146	399.680976	7.014182
5.466992	387.097836	7.019187
5.485708	403.287840	7.024192
5.801257	414.080686	7.029197
5.677637	410.650126	7.034202
5.342415	420.940832	7.039206
5.783354	422.046190	7.044211
5.872027	425.586675	7.049216
5.866776	410.319185	7.054221
5.685427	426.905331	7.059226
5.486963	421.472588	7.064230
5.727468	413.302615	7.069235
5.511485	429.299495	7.074240
5.789321	427.223129	7.079245
6.021786	418.769762	7.084250
5.642594	430.785434	7.089254
6.047580	421.471195	7.094259
5.713378	408.158475	7.099264
5.724480	404.236841	7.104269
5.330700	408.627750	7.109274
5.787756	415.362593	7.114278
5.903373	409.088310	7.119283
5.818611	417.429920	7.124288
5.626088	414.184380	7.129293
5.891477	406.672869	7.134298
5.480587	408.855044	7.139302
5.891543	409.675703	7.144307
5.514977	393.739247	7.149312
5.840400	406.513233	7.154317
5.628213	414.200503	7.159322
5.705769	424.355318	7.164326
5.785234	414.355159	7.169331
5.594768	429.090949	7.174336
5.694183	415.077337	7.179341
5.787829	416.517310	7.184346
5.534131	414.853761	7.189350
5.762454	419.706765	7.194355
5.864269	425.392713	7.199360
5.780713	424.555205	7.204365
5.924875	424.580002	7.209370
5.631226	402.888468	7.214374
5.769679	381.833014	7.219379
5.503629	400.482695	7.224384
5.514012	402.447068	7.229389
6.237518	413.057954	7.234394
5.807261	402.706180	7.239398
5.686253	382.849846	7.244403
5.386942	390.836913	7.249408
5.682307	392.891221	7.254413
5.921430	401.202678	7.259418
5.758738	394.954861	7.264422
5.750519	389.618843	7.269427
5.602048	394.430718	7.274432
5.281792	393.234945	7.279437
5.739720	402.484563	7.284442
5.511577	413.888654	7.289446
5.732279	404.075495	7.294451
5.373534	427.629306	7.299456
6.328489	409.792776	7.304461
6.272744	415.408076	7.309466
5.571169	401.204640	7.314470
5.524914	382.851005	7.319475
5.180605	394.442684	7.324480
5.745557	411.922222	7.329485
5.780830	422.846631	7.334490
5.864325	420.165857	7.339494
5.906057	413.631987	7.344499
5.740627	409.614232	7.349504
5.797458	420.482987	7.354509
5.953772	389.308127	7.359514
5.513714	396.045111	7.364518
5.502636	393.761867	7.369523
5.676706	407.611942	7.374528
5.690953	411.073665	7.379533
5.942007	417.289391	7.384538
5.939456	396.652827	7.389542
6.167419	392.782668	7.394547
5.732865	387.982662	7.399552
5.634831	389.901319	7.404557
5.774907	381.410853	7.409562
5.499315	382.551259	7.414566
5.713772	378.363198	7.419571
5.522423	389.962251	7.424576
5.715699	384.940498	7.429581
5.757151	382.666826	7.434586
5.286172	381.590475	7.439590
5.730261	392.946793	7.444595
5.738912	413.838124	7.449600
6.011883	412.741820	7.454605
5.837512	384.229680	7.459610
5.663266	387.496824	7.464614
5.687812	398.690148	7.469619
5.552229	393.564792	7.474624
5.652023	388.567860	7.479629
5.703227	394.213819	7.484634
5.583303	384.864905	7.489638
5.549516	400.046150	7.494643
5.817949	418.931114	7.499648
5.720846	421.677341	7.504653
6.182536	412.760494	7.509658
5.732937	403.584142	7.514662
5.758028	395.730058	7.519667
5.686926	390.088439	7.524672
5.338766	381.620848	7.529677
5.793367	395.272622	7.534682
5.666716	404.425979	7.539686
5.835934	403.888934	7.544691
5.651498	403.095427	7.549696
5.642904	388.098433	7.554701
5.934460	408.072172	7.559706
5.896475	403.721014	7.564710
5.726293	384.526595	7.569715
5.786595	396.529197	7.574720
5.684431	389.999681	7.579725
5.512068	382.421323	7.584730
5.367208	389.436364	7.589734
5.751593	408.136510	7.594739
5.699003	413.767369	7.599744
5.872852	417.403087	7.604749
5.705757	409.194520	7.609754
5.586463	416.473001	7.614758
5.692261	411.967459	7.619763
5.769731	423.211642	7.624768
5.682356	418.250466	7.629773
5.396559	415.673145	7.634778
5.753426	432.911353	7.639782
6.033880	416.641161	7.644787
5.988691	425.122935	7.649792
5.471871	414.222135	7.654797
5.390074	401.448691	7.659802
5.522256	422.502131	7.664806
6.304118	418.540427	7.669811
5.703274	425.618115	7.674816
5.632515	420.096097	7.679821
5.599760	411.976513	7.684826
5.834300	422.434892	7.689830
5.933125	412.192197	7.694835
5.618329	414.550081	7.699840
5.675443	410.283637	7.704845
5.765297	404.043111	7.709850
5.597934	409.988016	7.714854
5.710986	416.550631	7.719859
5.620552	419.740298	7.724864
5.767973	413.548561	7.729869
6.043677	417.261958	7.734874
5.757213	416.011665	7.739878
5.663054	396.714495	7.744883
5.778291	401.563887	7.749888
5.550665	390.126670	7.754893
5.809082	386.146708	7.759898
5.588816	392.329031	7.764902
5.719680	387.886834	7.769907
5.710560	397.341887	7.774912
5.885370	404.635687	7.779917
6.005339	403.595647	7.784922
5.854405	397.114341	7.789926
6.089511	390.732121	7.794931
5.956574	398.541049	7.799936
6.105621	391.483843	7.804941
5.993197	389.311564	7.809946
5.905681	392.556287	7.814950
5.585252	382.989332	7.819955
5.421767	388.813919	7.824960
5.684100	392.006448	7.829965
5.793840	382.168034	7.834970
5.616818	397.312373	7.839974
5.853311	398.099612	7.844979
5.740468	392.725340	7.849984
5.435469	385.035321	7.854989
5.466283	389.288575	7.859994
5.442607	397.464203	7.864998
5.613168	377.629243	7.870003
5.538323	400.036283	7.875008
5.669665	392.631381	7.880013
5.224440	389.297284	7.885018
5.263236	399.358747	7.890022
5.878077	398.150699	7.895027
5.697648	412.702993	7.900032
6.029067	421.508270	7.905037
5.804089	405.739326	7.910042
5.701649	401.866645	7.915046
5.405209	388.879874	7.920051
5.738131	403.079077	7.925056
5.768222	407.789429	7.930061
6.119427	382.779623	7.935066
5.595977	400.785891	7.940070
5.551168	388.552403	7.945075
5.436618	383.208408	7.950080
5.683192	408.679558	7.955085
6.028952	410.141302	7.960090
5.714364	400.995223	7.965094
5.582110	393.384383	7.970099
5.489004	395.188870	7.975104
5.377291	413.038417	7.980109
5.650779	408.599479	7.985114
5.539308	420.647061	7.990118
5.912772	419.863129	7.995136
5.870236	419.700297	8.000154
5.919474	425.566370	8.005171
6.165813	412.435850	8.010189
5.793317	396.934032	8.015206
5.749471	380.579962	8.020224
5.600791	387.549853	8.025242
5.765100	387.424968	8.030259
6.016887	387.722539	8.035277
5.268040	388.270596	8.040294
6.191576	394.306471	8.045312
5.810262	391.526388	8.050330
5.737029	388.769884	8.055347
5.830073	373.860694	8.060365
5.673681	381.035847	8.065382
6.040348	378.501268	8.070400
6.093612	388.152449	8.075418
5.697292	392.166480	8.080435
5.848783	378.619571	8.085453
5.854088	380.264973	8.090470
6.110162	386.183346	8.095488
5.857258	382.071798	8.100506
5.762095	379.379733	8.105523
5.793190	387.865640	8.110541
5.306072	390.748075	8.115558
5.620504	383.177064	8.120576
5.668293	401.761466	8.125594
5.433075	399.233556	8.130611
6.224119	408.641000	8.135629
5.551968	410.960839	8.140646
6.123383	409.727266	8.145664
6.126541	417.814351	8.150682
5.767787	396.476779	8.155699
5.660028	396.607637	8.160717
6.086217	415.489186	8.165734
5.983015	411.585025	8.170752
5.679936	413.347620	8.175770
5.811492	418.846029	8.180787
6.411342	405.779900	8.185805
5.742460	409.840456	8.190822
5.951474	414.999066	8.195840
6.049153	423.040815	8.200858
5.810153	398.500474	8.205875
5.926807	397.879539	8.210893
6.010833	403.649421	8.215910
6.012878	397.159825	8.220928
5.725006	397.883417	8.225946
5.994381	417.767346	8.230963
6.187937	416.055784	8.235981
5.844364	410.298056	8.240998
6.355349	407.520377	8.246016
6.293969	392.542615	8.251034
5.817748	386.247195	8.256051
5.808930	382.186923	8.261069
5.582960	383.183589	8.266086
5.942423	394.433024	8.271104
5.846634	410.546530	8.276122
6.050091	420.936820	8.281139
6.327115	416.157792	8.286157
6.207897	419.301902	8.291174
5.850625	417.083566	8.296192
6.162937	402.521690	8.301210
5.928136	404.780075	8.306227
6.157581	410.231799	8.311245
6.224715	401.739060	8.316262
6.072374	391.615637	8.321280
6.091468	386.397656	8.326298
5.747092	394.294086	8.331315
6.123669	391.091377	8.336333
5.925170	420.932966	8.341350
5.962755	419.265482	8.346368
6.166542	406.199172	8.351386
5.952055	428.696880	8.356403
6.203173	409.919641	8.361421
5.743576	415.423933	8.366438
6.221629	418.540090	8.371456
5.995931	417.210444	8.376474
6.021206	419.207197	8.381491
5.752487	427.899136	8.386509
6.079635	429.759407	8.391526
6.283325	420.984107	8.396544
6.367588	420.974298	8.401562
6.168908	422.391857	8.406579
6.183374	403.141445	8.411597
6.117538	420.744274	8.416614
6.193632	429.284073	8.421632
6.059940	421.516293	8.426650
5.964512	427.197362	8.431667
5.975348	418.549584	8.436685
6.098525	425.582908	8.441702
6.136475	416.666533	8.446720
6.211568	419.708664	8.451738
6.128012	431.955355	8.456755
6.409015	411.900811	8.461773
6.101091	422.278489	8.466790
5.895172	434.026420	8.471808
5.951217	423.840787	8.476826
5.870351	423.720601	8.481843
6.066221	420.416578	8.486861
6.110947	432.162152	8.491878
5.970831	437.316572	8.496896
6.242223	447.130716	8.501914
5.790186	459.355762	8.506931
6.479668	448.549202	8.511949
6.262671	458.906859	8.516966
6.155042	450.550925	8.521984
6.367352	453.267105	8.527002
6.174316	463.990215	8.532019
6.567105	453.445433	8.537037
6.572914	451.455905	8.542054
6.351632	442.159121	8.547072
6.864561	446.641273	8.552090
6.143347	441.346546	8.557107
6.346322	418.350206	8.562125
6.060244	419.861424	8.567143
6.006039	449.176573	8.572160
6.391837	445.396862	8.577178
6.057622	450.012422	8.582195
6.577438	444.058366	8.587213
6.750178	456.668834	8.592231
6.624430	451.531744	8.597248
6.818353	418.336229	8.602266
6.112573	422.818346	8.607283
6.109330	420.834058	8.612301
6.357970	423.030067	8.617319
6.277218	429.114333	8.622336
6.326406	444.623430	8.627354
6.315461	452.394821	8.632371
6.261217	438.402927	8.637389
6.632030	444.255717	8.642407
6.369919	448.673673	8.647424
6.575007	442.881645	8.652442
6.478574	451.999655	8.657459
6.323454	440.028234	8.662477
6.169611	441.109322	8.667495
6.393090	452.093539	8.672512
6.410062	455.831160	8.677530
6.423786	455.879259	8.682547
6.447102	457.019142	8.687565
6.513016	452.286307	8.692583
6.086656	447.608259	8.697600
6.328847	451.604461	8.702618
6.271153	459.739904	8.707635
6.401137	447.531736	8.712653
6.735856	454.185207	8.717671
6.546314	459.293581	8.722688
6.654408	450.917446	8.727706
6.318587	455.732738	8.732723
6.549971	452.508648	8.737741
6.555689	456.077692	8.742759
6.347275	452.793634	8.747776
6.278927	448.692603	8.752794
6.157620	462.018063	8.757811
6.534005	446.991716	8.762829
6.736784	452.033777	8.767847
6.340617	459.319935	8.772864
6.577800	446.033945	8.777882
6.666718	451.724707	8.782899
6.584440	446.410392	8.787917
6.376560	450.606832	8.792935
6.445642	455.423404	8.797952
6.616432	457.914508	8.802970
6.307309	447.469886	8.807987
6.609794	437.276876	8.813005
6.649969	442.525787	8.818023
6.153394	446.023246	8.823040
6.874558	463.743648	8.828058
6.796132	482.247059	8.833075
6.841278	470.399080	8.838093
7.020833	462.799445	8.843111
6.584085	461.103577	8.848128
6.741828	449.245666	8.853146
6.185978	452.314827	8.858163
6.555173	459.661863	8.863181
6.813651	455.244965	8.868199
6.717812	445.923904	8.873216
6.869361	453.334950	8.878234
6.574299	450.601122	8.883251
6.758821	443.128010	8.888269
6.459199	457.506928	8.893287
6.265488	466.701148	8.898304
6.522150	479.063858	8.903322
6.693133	488.277922	8.908339
6.989484	489.930539	8.913357
7.173353	486.955680	8.918375
6.835917	476.999571	8.923392
7.240865	464.613595	8.928410
6.695563	451.062806	8.933427
6.629270	459.790980	8.938445
6.348085	463.454084	8.943463
6.681971	448.730365	8.948480
6.933728	459.915382	8.953498
6.986242	462.413142	8.958515
6.988869	449.940746	8.963533
6.890917	453.387090	8.968551
6.685884	462.835388	8.973568
6.911314	450.137628	8.978586
6.746767	453.407617	8.983603
6.371154	461.437464	8.988621
7.029887	463.744508	8.993639
7.099101	460.389572	8.998656
7.154328	453.994291	9.003674
7.139775	453.840217	9.008691
6.680477	451.554798	9.013709
6.992232	456.014503	9.018727
6.903001	455.812350	9.023744
7.129248	454.314134	9.028762
6.902927	463.811807	9.033779
6.635859	455.331759	9.038797
6.986339	450.859607	9.043815
6.857431	459.437140	9.048832
6.897660	449.300551	9.053850
6.592660	451.101845	9.058867
6.635184	457.575209	9.063885
6.884821	445.507471	9.068903
6.416442	460.170821	9.073920
6.686010	459.356537	9.078938
6.779786	470.761232	9.083955
7.021914	488.884580	9.088973
7.223998	496.574833	9.093991
7.044517	484.844559	9.099008
7.483299	461.054916	9.104026
7.171792	473.669261	9.109043
6.970643	467.029396	9.114061
6.812066	457.745167	9.119079
6.603573	465.100882	9.124096
6.841797	454.701795	9.129114
6.843279	457.037355	9.134131
7.189065	467.649280	9.139149
7.117433	463.741463	9.144167
6.792175	463.074487	9.149184
7.072785	457.009301	9.154202
7.078496	474.300824	9.159219
7.080235	466.362837	9.164237
7.235588	455.256731	9.169255
7.018803	464.971680	9.174272
7.167029	448.402172	9.179290
6.844340	455.003692	9.184307
6.863649	453.605409	9.189325
7.129820	466.548008	9.194343
7.077508	478.326974	9.199360
7.604359	463.311071	9.204378
7.271021	471.697738	9.209395
6.837243	458.485128	9.214413
7.223687	459.149636	9.219431
6.781707	463.148106	9.224448
6.729841	452.888378	9.229466
6.973891	484.360723	9.234483
6.844558	492.626894	9.239501
7.252016	495.251690	9.244519
6.995679	497.296371	9.249536
7.126110	493.976971	9.254554
7.305504	501.289954	9.259571
7.099045	486.750654	9.264589
7.524955	488.523366	9.269607
7.222269	491.280773	9.274624
7.457956	492.698488	9.279642
6.958154	488.008947	9.284659
7.205663	494.152352	9.289677
7.500269	486.333242	9.294695
7.146472	472.785718	9.299712
6.942137	486.915206	9.304730
7.171295	486.746146	9.309747
7.157400	479.855101	9.314765
7.337239	483.624265	9.319783
6.986911	493.838563	9.324800
7.302081	480.050879	9.329818
7.342461	477.975927	9.334835
7.251011	491.658115	9.339853
7.624045	483.945902	9.344871
7.184424	501.267557	9.349888
7.156361	490.017070	9.354906
7.361765	488.849588	9.359923
7.403281	497.489313	9.364941
7.462642	483.873008	9.369959
7.230240	483.132331	9.374976
7.202524	493.356784	9.379994
7.190393	487.939444	9.385011
6.837691	500.794625	9.390029
7.387350	492.354251	9.395047
7.116633	491.634666	9.400064
7.411506	489.469142	9.405082
7.205597	489.721022	9.410099
7.215248	487.331627	9.415117
7.449160	479.958778	9.420135
7.300235	491.125506	9.425152
6.716851	482.341198	9.430170
6.973844	489.102391	9.435187
7.067739	498.413041	9.440205
7.610266	494.403129	9.445223
7.233907	492.401671	9.450240
7.066935	494.560689	9.455258
7.645462	512.213597	9.460275
7.390727	509.280417	9.465293
7.914068	508.194812	9.470311
7.371099	505.453725	9.475328
7.294787	495.562006	9.480346
7.309988	494.330210	9.485363
7.253507	513.381293	9.490381
7.644345	505.477288	9.495399
7.455066	517.838152	9.500416
7.459943	513.435889	9.505434
7.748148	507.025012	9.510451
7.455986	512.330640	9.515469
7.828364	497.002509	9.520487
7.419893	497.100700	9.525504
7.307133	486.951188	9.530522
7.523463	501.435391	9.535539
7.511249	504.753035	9.540557
7.835802	502.579061	9.545575
7.357209	502.422459	9.550592
7.253538	494.763830	9.555610
7.421755	496.053846	9.560627
7.434571	502.580555	9.565645
7.452712	505.503008	9.570663
7.429366	511.975375	9.575680
7.363499	521.333401	9.580698
7.819174	513.720976	9.585715
7.531798	513.687366	9.590733
7.362729	513.921744	9.595751
7.542101	507.877007	9.600768
7.692849	514.589445	9.605786
7.901832	516.291339	9.610803
7.571274	522.377958	9.615821
7.766835	510.934429	9.620839
7.938389	511.314244	9.625856
7.456948	515.153437	9.630874
7.757262	513.034440	9.635891
7.875929	514.467757	9.640909
7.835223	510.574104	9.645927
7.750110	517.206157	9.650944
7.871151	513.130098	9.655962
7.835278	515.305437	9.660979
7.695786	515.685584	9.665997
7.637156	499.729613	9.671015
7.809565	505.829048	9.676032
7.485886	512.971489	9.681050
7.923593	514.088946	9.686067
7.639014	506.628578	9.691085
7.899155	510.215419	9.696103
7.719845	511.618075	9.701120
7.729571	513.578835	9.706138
7.928786	511.906083	9.711155
7.507582	508.656195	9.716173
7.857735	512.335225	9.721191
7.537515	509.452918	9.726208
7.399573	534.270712	9.731226
7.689519	522.351240	9.736243
7.501412	516.994166	9.741261
7.838719	515.903977	9.746279
8.013313	526.344965	9.751296
7.793156	521.717642	9.756314
7.890545	511.705691	9.761331
7.561371	514.100725	9.766349
7.811323	524.515679	9.771367
7.907693	516.046780	9.776384
7.846806	522.324019	9.781402
7.503777	513.505483	9.786419
7.801677	520.466284	9.791437
7.788940	517.560713	9.796455
7.877450	522.595210	9.801472
7.719146	515.765900	9.806490
7.907743	521.890417	9.811507
7.498655	522.604328	9.816525
7.722266	513.302171	9.821543
8.066229	529.231143	9.826560
7.783557	536.737901	9.831578
8.182344	534.009445	9.836595
7.917801	527.439762	9.841613
7.571950	523.535623	9.846631
8.021790	541.664166	9.851648
7.916009	544.535173	9.856666
8.204929	546.609509	9.861683
8.287854	544.164403	9.866701
8.319937	536.804117	9.871719
8.212118	522.675164	9.876736
7.735889	518.615346	9.881754
8.082681	516.226616	9.886771
7.971439	524.822620	9.891789
8.122453	507.218454	9.896807
8.084790	513.063496	9.901824
7.945016	523.755508	9.906842
8.155175	512.515331	9.911859
7.615199	510.021038	9.916877
7.888665	523.073086	9.921895
7.866458	523.037871	9.926912
8.022878	536.463235	9.931930
8.254671	545.695132	9.936947
8.068677	551.484010	9.941965
8.254346	554.711396	9.946983
8.436596	546.857783	9.952000
7.996092	529.801155	9.957018
8.385998	517.891342	9.962035
8.114346	527.194226	9.967053
7.810166	519.460377	9.972071
8.384897	522.779627	9.977088
8.235976	531.068638	9.982106
8.005561	515.836269	9.987123
8.337264	530.571849	9.992141
8.084194	522.243454	9.997159
8.198431	534.214971	10.002176
7.860698	528.212780	10.007194
8.186781	537.432533	10.012211
8.161775	543.550734	10.017229
8.275133	550.476705	10.022247
8.327413	545.039253	10.027264
7.830432	560.304840	10.032282
8.253377	551.265916	10.037299
8.305632	552.563096	10.042317
8.325526	548.364500	10.047335
8.467360	550.091272	10.052352
8.442551	562.925774	10.057370
8.344173	540.550885	10.062387
8.388464	557.420760	10.067405
7.989586	545.214303	10.072423
8.331056	536.222901	10.077440
8.288421	546.412362	10.082458
8.326203	539.663605	10.087475
8.147238	556.804676	10.092493
8.284458	549.578454	10.097511
8.344097	547.340304	10.102528
8.099217	559.445386	10.107546
8.139247	552.160831	10.112563
8.115519	556.341824	10.117581
8.401301	554.561965	10.122599
8.255753	551.043527	10.127616
8.379030	553.464070	10.132634
8.187141	558.937062	10.137651
8.006015	556.713015	10.142669
8.482092	545.294250	10.147687
8.454664	555.719639	10.152704
8.418945	558.618727	10.157722
8.360525	552.547635	10.162739
8.321288	549.616424	10.167757
7.998109	551.216347	10.172775
8.394882	555.686632	10.177792
8.382034	559.326964	10.182810
8.707132	556.010805	10.187827
8.285955	559.731509	10.192845
8.486272	561.491719	10.197863
8.699190	568.712401	10.202880
8.532932	565.005690	10.207898
8.479126	562.465780	10.212915
8.500512	566.530387	10.217933
8.459903	569.504187	10.222951
8.786924	551.795013	10.227968
8.540690	558.617063	10.232986
8.593403	555.712280	10.238003
8.562811	559.771797	10.243021
8.713659	552.623423	10.248039
8.661628	553.134362	10.253056
8.459031	561.439838	10.258074
8.333280	553.753929	10.263091
8.713850	554.395598	10.268109
8.206777	561.355224	10.273127
8.201228	572.748757	10.278144
8.625634	577.441404	10.283162
8.639875	577.025340	10.288179
8.629260	589.718570	10.293197
8.553727	588.530495	10.298215
8.467146	581.762614	10.303232
8.549364	591.229746	10.308250
8.321503	582.969971	10.313267
8.160272	587.588868	10.318285
8.567631	589.730725	10.323303
8.670559	583.444707	10.328320
8.690785	586.396747	10.333338
8.533781	584.930759	10.338355
8.654496	578.478451	10.343373
8.414837	579.163775	10.348391
8.779875	596.324906	10.353408
8.691398	585.413597	10.358426
8.529430	597.527148	10.363443
9.043764	611.688345	10.368461
8.828861	600.373497	10.373479
8.855215	581.605050	10.378496
8.435398	593.469833	10.383514
8.740918	607.699780	10.388531
8.972169	616.798766	10.393549
8.691341	630.118851	10.398567
8.802333	630.108069	10.403584
8.785487	620.992406	10.408602
8.765044	618.921583	10.413619
8.701784	626.242647	10.418637
8.758417	626.644803	10.423655
9.128086	617.338913	10.428672
8.861004	616.846825	10.433690
8.986490	611.136970	10.438707
9.149623	619.813543	10.443725
8.749107	601.158424	10.448743
9.079618	598.250629	10.453760
8.648207	591.967793	10.458778
8.875363	609.182723	10.463795
8.984303	616.746234	10.468813
8.512791	611.913130	10.473831
8.930283	620.387267	10.478848
8.771336	624.096336	10.483866
8.932717	608.961593	10.488883
8.813754	616.818424	10.493901
8.918072	613.846453	10.498919
9.153295	609.911997	10.503936
8.778355	622.336003	10.508954
8.583515	622.076808	10.513971
8.881353	613.828249	10.518989
8.933121	620.326724	10.524007
9.237505	614.915485	10.529024
8.811810	619.741351	10.534042
9.137172	617.620169	10.539059
8.910252	615.584551	10.544077
8.853991	617.722535	10.549095
9.124948	615.127667	10.554112
9.090477	626.338656	10.559130
9.159858	609.659983	10.564147
9.111568	609.922423	10.569165
8.960036	626.311060	10.574183
9.010162	624.456775	10.579200
9.387738	624.215657	10.584218
9.168765	615.242630	10.589235
9.220912	617.978420	10.594253
8.775826	620.935331	10.599271
9.269918	622.081759	10.604288
8.890481	622.187452	10.609306
8.864655	619.662886	10.614323
9.030124	611.408158	10.619341
8.797237	628.937081	10.624359
9.440549	622.735232	10.629376
9.239615	638.084521	10.634394
9.189131	653.152125	10.639411
9.139869	636.393050	10.644429
9.283952	646.511177	10.649447
9.178438	647.702083	10.654464
9.423718	651.806665	10.659482
9.475742	645.163852	10.664499
9.198738	626.542019	10.669517
9.130580	621.195099	10.674535
9.283204	621.241401	10.679552
9.332213	620.122585	10.684570
8.999899	635.241765	10.689587
9.412609	635.018851	10.694605
9.229166	638.853798	10.699623
9.650644	644.478651	10.704640
9.216951	645.158846	10.709658
9.464495	638.181522	10.714675
9.545551	634.423688	10.719693
9.202487	626.929037	10.724711
9.095708	615.048783	10.729728
9.137055	635.424916	10.734746
9.486916	644.971447	10.739763
9.613454	645.640833	10.744781
9.409160	652.689411	10.749799
9.431156	641.480530	10.754816
9.316112	631.919961	10.759834
9.143120	648.617816	10.764851
9.289360	644.625925	10.769869
9.044701	650.655001	10.774887
9.218269	657.869731	10.779904
8.935407	649.399664	10.784922
9.428231	658.526693	10.789939
9.143121	650.273883	10.794957
9.041729	643.944457	10.799975
8.989843	649.974345	10.804992
9.222982	666.416458	10.810010
9.362565	677.613284	10.815027
9.662728	677.960237	10.820045
9.304624	681.455431	10.825063
9.388268	680.791229	10.830080
9.449707	680.926798	10.835098
9.158288	689.248301	10.840115
9.482578	685.563030	10.845133
9.388288	683.460120	10.850151
9.743605	688.248060	10.855168
9.826735	681.666810	10.860186
9.719136	685.059988	10.865203
9.699990	670.819315	10.870221
9.693122	691.865269	10.875239
10.153464	685.161848	10.880256
9.855166	694.019128	10.885274
9.429307	687.930670	10.890291
9.946440	678.403858	10.895309
10.157338	674.658015	10.900327
9.925321	669.820935	10.905344
9.862960	652.182687	10.910362
9.453454	665.638415	10.915379
9.562941	646.225470	10.920397
9.752721	658.533447	10.925415
9.834349	656.459920	10.930432
9.583742	650.772743	10.935450
9.544755	650.013379	10.940467
9.607144	662.741348	10.945485
9.617427	674.380912	10.950503
9.787607	679.078210	10.955520
10.148054	675.457425	10.960538
9.913963	669.297723	10.965555
9.602634	651.344491	10.970573
9.380330	661.448095	10.975591
10.056119	674.279779	10.980608
10.140925	674.725991	10.985626
9.604998	669.913452	10.990643
9.762611	662.401974	10.995661
9.751215	668.624646	11.000679
10.004406	672.224188	11.005696
9.872033	678.396103	11.010714
9.868060	684.852252	11.015731
9.986763	683.043604	11.020749
10.065263	679.650775	11.025767
9.602727	671.418222	11.030784
10.042609	668.610524	11.035802
9.724050	672.453539	11.040819
10.237942	670.708298	11.045837
9.724041	673.975942	11.050855
9.767493	683.827611	11.055872
9.359527	681.240327	11.060890
9.667448	693.111666	11.065907
9.976351	685.956200	11.070925
9.783618	693.025224	11.075943
9.915118	686.496694	11.080960
9.956234	682.668890	11.085978
9.541963	682.936509	11.090995
9.689767	679.445925	11.096013
9.672633	678.739039	11.101031
9.959288	692.857245	11.106048
10.222215	699.881180	11.111066
10.066431	708.681852	11.116083
10.124745	696.972046	11.121101
9.989658	701.516690	11.126119
9.974971	701.884088	11.131136
10.297376	696.594620	11.136154
9.962183	708.420905	11.141171
10.047987	705.439871	11.146189
10.111703	712.330821	11.151207
10.006292	721.336421	11.156224
10.360258	720.841085	11.161242
10.117122	716.269458	11.166259
10.333201	719.341193	11.171277
10.080313	700.528609	11.176295
10.251925	697.953688	11.181312
10.324840	699.834456	11.186330
9.946586	704.840464	11.191347
10.430080	699.730042	11.196365
9.806723	690.272925	11.201383
9.652310	704.967674	11.206400
10.504145	709.986595	11.211418
10.107094	718.281878	11.216435
10.198295	717.966553	11.221453
10.487355	721.427429	11.226471
10.212726	717.380097	11.231488
10.484524	713.832997	11.236506
10.218042	728.690258	11.241523
10.562174	709.294251	11.246541
10.486271	712.811798	11.251559
10.327908	718.822407	11.256576
10.328162	720.467794	11.261594
10.413957	716.226772	11.266611
10.622733	716.972218	11.271629
10.493703	704.048533	11.276647
9.759813	690.195200	11.281664
10.520412	701.121534	11.286682
10.084512	706.737048	11.291699
10.326430	707.009393	11.296717
10.612795	713.597163	11.301735
9.881438	711.850466	11.306752
10.240140	717.569070	11.311770
10.252279	718.744770	11.316787
10.214175	715.052859	11.321805
10.330272	714.324249	11.326823
10.058383	718.879992	11.331840
10.626496	705.772310	11.336858
10.321050	716.530705	11.341875
10.415313	714.764864	11.346893
10.755766	714.017185	11.351911
10.206066	713.169811	11.356928
10.693857	720.044411	11.361946
10.406932	726.335274	11.366963
10.512499	728.169222	11.371981
10.545787	719.302251	11.376999
10.516417	725.654172	11.382016
10.966510	717.264868	11.387034
10.980157	714.879206	11.392051
10.534143	721.787679	11.397069
10.673423	721.964409	11.402087
10.222298	726.414369	11.407104
10.421787	708.387083	11.412122
10.503695	719.919884	11.417139
10.581731	716.911004	11.422157
10.538780	717.694312	11.427175
10.496352	736.497531	11.432192
10.675655	740.445552	11.437210
10.701113	750.457196	11.442227
10.756168	757.078784	11.447245
11.127390	754.355632	11.452263
10.600867	730.825770	11.457280
10.965823	718.144291	11.462298
10.431363	727.685768	11.467315
11.007081	721.232700	11.472333
10.772729	715.786859	11.477351
10.705100	718.884323	11.482368
10.833478	723.464256	11.487386
10.595758	719.295197	11.492403
10.469567	718.650910	11.497421
10.733585	724.342752	11.502439
10.852916	742.947429	11.507456
10.604849	752.224016	11.512474
10.876941	756.523467	11.517491
10.524034	745.762514	11.522509
10.854776	756.221645	11.527527
10.722045	759.108757	11.532544
10.803852	754.213195	11.537562
10.501007	746.361809	11.542579
10.989396	751.055350	11.547597
10.737116	756.192396	11.552615
10.580903	750.972658	11.557632
10.899702	746.365625	11.562650
10.735456	759.695585	11.567667
10.891725	748.481166	11.572685
10.979083	751.756724	11.577703
10.704696	751.805202	11.582720
10.667629	751.963743	11.587738
11.014155	764.974598	11.592755
10.954467	769.431717	11.597773
10.953744	771.600595	11.602791
10.879275	793.033968	11.607808
11.126733	781.407286	11.612826
10.919274	788.783552	11.617843
10.682552	789.798552	11.622861
10.981698	782.762250	11.627879
10.731466	788.941682	11.632896
10.537010	783.312879	11.637914
10.905773	782.401002	11.642931
11.078514	782.581355	11.647949
11.396643	786.005460	11.652967
10.939741	791.232326	11.657984
11.205383	783.302521	11.663002
11.276117	786.576208	11.668019
10.835691	790.117308	11.673037
10.888810	779.902599	11.678055
11.069895	780.513478	11.683072
11.217499	782.748477	11.688090
11.061008	773.805379	11.693107
10.843673	782.115278	11.698125
11.398034	803.878520	11.703143
11.070511	814.601958	11.708160
11.206529	820.041911	11.713178
11.239335	819.558611	11.718195
11.313331	814.701617	11.723213
11.656983	809.747511	11.728231
10.961406	822.656572	11.733248
11.417792	819.401225	11.738266
11.814017	817.697751	11.743283
11.681835	807.316637	11.748301
11.584002	797.823973	11.753319
11.422763	781.405427	11.758336
11.101852	786.575868	11.763354
11.456052	789.873957	11.768371
11.330870	782.916046	11.773389
11.412985	781.381491	11.778407
11.155295	791.207126	11.783424
11.006086	780.158893	11.788442
11.182884	789.497644	11.793459
10.989162	790.410084	11.798477
11.334637	805.013657	11.803495
11.113846	820.473673	11.808512
11.432563	815.671690	11.813530
11.277284	816.052485	11.818547
11.268365	807.043353	11.823565
11.841111	814.344030	11.828583
11.338815	810.863429	11.833600
11.541815	805.375195	11.838618
11.464446	810.793432	11.843635
11.197167	823.667533	11.848653
11.328180	815.965137	11.853671
11.331671	814.936786	11.858688
11.384866	809.708204	11.863706
11.476971	816.634167	11.868723
11.544341	824.686154	11.873741
11.906076	808.915954	11.878759
11.388341	827.869868	11.883776
11.262569	813.515902	11.888794
11.449663	816.184355	11.893811
11.885073	833.551601	11.898829
11.888158	825.486851	11.903847
11.663223	814.380649	11.908864
11.687018	824.680946	11.913882
11.286384	828.832882	11.918899
11.411061	834.875880	11.923917
11.965364	836.640110	11.928935
11.542240	857.011225	11.933952
11.756057	850.121450	11.938970
11.771444	851.796824	11.943987
11.547725	856.385485	11.949005
11.622424	849.505318	11.954023
11.487332	851.504913	11.959040
11.546218	856.787087	11.964058
11.751214	847.955532	11.969075
11.603599	853.623636	11.974093
12.002329	851.632791	11.979111
11.889855	854.120486	11.984128
11.882413	849.249779	11.989146
12.092519	859.143888	11.994163
12.051729	850.592374	11.999181
12.299865	847.188302	12.004199
12.088857	864.722832	12.009216
12.086898	858.242264	12.014234
11.939661	833.043763	12.019251
11.659303	831.614866	12.024269
12.083929	833.116918	12.029287
11.912882	827.093655	12.034304
11.938992	836.757282	12.039322
11.913870	843.049308	12.044339
11.811241	856.448386	12.049357
12.088123	848.709566	12.054375
11.849780	854.730002	12.059392
12.054566	856.421312	12.064410
12.136898	854.558823	12.069427
12.063607	856.667869	12.074445
11.965930	854.591178	12.079463
11.838905	855.847750	12.084480
11.891575	863.213240	12.089498
12.026157	854.885057	12.094515
11.950893	859.665582	12.099533
12.276862	836.545556	12.104551
12.009055	854.681673	12.109568
11.612541	858.968146	12.114586
11.995542	852.112013	12.119603
12.052468	868.334495	12.124621
12.047372	857.041172	12.129639
11.870627	853.592276	12.134656
11.643277	845.826572	12.139674
11.888135	855.359983	12.144691
11.910147	873.782219	12.149709
12.265601	881.559798	12.154727
12.180429	896.250471	12.159744
12.181259	898.298758	12.164762
12.270162	891.581647	12.169779
12.232683	885.985417	12.174797
12.346648	883.386534	12.179815
12.339461	880.362381	12.184832
12.326702	891.200654	12.189850
12.319322	893.253053	12.194867
12.059076	892.599127	12.199885
12.447613	882.138894	12.204903
12.163623	877.281898	12.209920
12.052084	886.323541	12.214938
11.909487	894.910860	12.219955
11.681310	886.484667	12.224973
12.008125	892.693261	12.229991
11.810929	889.938652	12.235008
12.238471	904.880071	12.240026
12.965031	910.638430	12.245043
12.745500	909.516737	12.250061
12.614499	892.880614	12.255079
12.603729	891.777169	12.260096
12.252189	892.332794	12.265114
12.787363	888.008702	12.270131
12.429575	883.042466	12.275149
12.621460	887.063334	12.280167
12.422075	899.103891	12.285184
12.245571	891.463693	12.290202
12.399682	887.666859	12.295219
12.199189	897.879886	12.300237
12.518982	902.930607	12.305255
12.597567	913.123305	12.310272
12.436133	918.682221	12.315290
12.498813	912.475640	12.320307
12.310783	925.807017	12.325325
12.627203	914.285845	12.330343
12.460648	915.167528	12.335360
12.334636	917.758633	12.340378
12.424242	914.121146	12.345395
12.423802	923.514757	12.350413
12.721140	919.541223	12.355431
12.784515	913.557518	12.360448
12.348002	914.352539	12.365466
12.754540	912.014889	12.370483
12.602381	917.869756	12.375501
12.505961	918.032990	12.380519
12.894239	918.809204	12.385536
12.652368	935.274899	12.390554
12.919873	910.495732	12.395571
12.564110	916.173163	12.400589
12.700539	941.399238	12.405607
13.211702	939.339713	12.410624
12.559732	929.214660	12.415642
12.568734	933.549865	12.420659
12.684866	945.843477	12.425677
12.781117	939.791544	12.430695
12.996977	945.113642	12.435712
12.907997	953.137902	12.440730
13.029242	944.611222	12.445747
12.731275	948.813631	12.450765
12.707251	953.442732	12.455783
13.197656	951.584434	12.460800
13.201123	963.348156	12.465818
13.393612	955.932131	12.470835
12.889075	936.068721	12.475853
12.822644	923.000476	12.480871
12.713902	933.543772	12.485888
12.645936	944.484102	12.490906
13.108424	945.702794	12.495923
13.049342	954.981138	12.500941
13.152984	958.458343	12.505959
12.983971	951.903393	12.510976
12.798215	957.642885	12.515994
12.956738	953.858690	12.521011
12.795402	953.847646	12.526029
12.801625	956.971627	12.531047
13.131096	955.970089	12.536064
12.853177	950.204357	12.541082
13.117793	948.936423	12.546099
13.115305	951.229218	12.551117
13.284851	952.108302	12.556135
13.483772	948.338982	12.561152
12.940333	951.704461	12.566170
13.022357	952.540145	12.571187
13.174120	965.057075	12.576205
13.240748	945.854046	12.581223
13.325589	955.177491	12.586240
13.328711	965.232427	12.591258
13.569974	947.373222	12.596275
13.266398	950.187539	12.601293
13.169334	950.050343	12.606311
13.361998	951.935266	12.611328
13.387631	968.061074	12.616346
13.605074	934.315579	12.621363
13.298000	952.633465	12.626381
13.167590	951.683129	12.631399
13.556938	948.925458	12.636416
13.427781	950.221359	12.641434
13.260617	947.241246	12.646451
13.504870	954.824975	12.651469
13.087894	959.818077	12.656487
13.510548	954.428505	12.661504
13.040509	947.344670	12.666522
13.248594	954.881926	12.671539
13.220409	961.670184	12.676557
13.798991	970.981814	12.681575
13.841541	976.461871	12.686592
13.634096	962.129234	12.691610
13.720710	953.141821	12.696627
13.443626	958.227236	12.701645
13.434254	950.541281	12.706663
13.638570	949.120841	12.711680
13.241525	956.439262	12.716698
13.461328	948.135225	12.721715
13.455121	957.656559	12.726733
13.453566	983.725142	12.731751
13.599976	982.032332	12.736768
13.414193	986.537119	12.741786
13.490391	982.170467	12.746803
13.687384	988.338361	12.751821
13.444842	981.264444	12.756839
13.749302	990.419750	12.761856
13.422115	994.887978	12.766874
13.377452	984.869771	12.771891
13.314340	989.731483	12.776909
13.547403	997.689556	12.781927
13.799934	976.469113	12.786944
13.288372	989.568236	12.791962
14.045895	993.699457	12.796979
13.787401	998.358955	12.801997
13.666107	994.118818	12.807015
14.170183	999.610686	12.812032
13.617170	1000.258950	12.817050
13.655281	985.361986	12.822067
13.852706	998.528759	12.827085
13.895659	1014.559545	12.832103
14.393654	1012.046755	12.837120
13.893405	1002.263740	12.842138
13.872732	990.654839	12.847155
13.855674	988.875185	12.852173
13.912366	996.206813	12.857191
14.058154	986.209288	12.862208
13.760869	982.998650	12.867226
13.862362	985.267475	12.872243
14.414846	994.903060	12.877261
13.953046	990.956654	12.882279
14.012137	975.521484	12.887296
13.703342	987.517604	12.892314
14.065848	996.096099	12.897331
14.194331	998.606977	12.902349
13.889217	1001.517899	12.907367
14.274217	1008.857765	12.912384
13.989807	1005.591264	12.917402
14.200134	1013.240461	12.922419
14.391110	1011.307154	12.927437
14.018633	998.935764	12.932455
14.443880	990.578367	12.937472
13.977796	988.658784	12.942490
13.933329	983.127835	12.947507
14.168532	994.219834	12.952525
14.079396	1005.667652	12.957543
14.609456	1004.955740	12.962560
14.427663	1018.080887	12.967578
14.097843	999.751039	12.972595
14.324517	993.475009	12.977613
14.043921	1015.359709	12.982631
14.529954	1009.925792	12.987648
14.142967	1016.988293	12.992666
14.359512	1018.724618	12.997683
14.317934	1019.019414	13.002701
14.332629	1017.917952	13.007719
14.437316	1011.521547	13.012736
13.766407	1015.097934	13.017754
13.899025	1019.634546	13.022771
14.261271	1014.895964	13.027789
14.231469	1015.524582	13.032807
14.276508	1015.957989	13.037824
14.076141	1020.555929	13.042842
14.135362	1015.765180	13.047859
14.184538	1010.568881	13.052877
14.428512	1022.085064	13.057895
14.411120	1036.755320	13.062912
14.530538	1043.434788	13.067930
14.553145	1037.040031	13.072947
14.751653	1032.942962	13.077965
14.538035	1048.370235	13.082983
14.556133	1042.748035	13.088000
14.531783	1041.813034	13.093018
14.728982	1044.800963	13.098035
14.781023	1030.480980	13.103053
14.342008	1047.495819	13.108071
14.268705	1044.518971	13.113088
14.350696	1039.349124	13.118106
14.284618	1036.267559	13.123123
14.610805	1038.333245	13.128141
13.926587	1035.926765	13.133159
14.560038	1031.940168	13.138176
14.491812	1040.405061	13.143194
14.719909	1043.453029	13.148211
14.771850	1048.734941	13.153229
14.677632	1063.098683	13.158247
14.593864	1059.716054	13.163264
14.843834	1074.584934	13.168282
14.578518	1079.056148	13.173299
14.920551	1072.420530	13.178317
14.804903	1086.728003	13.183335
15.131756	1089.061749	13.188352
14.971527	1077.166451	13.193370
14.929191	1064.898000	13.198387
14.595789	1068.256642	13.203405
14.483152	1072.262836	13.208423
14.938045	1065.862856	13.213440
14.896452	1073.514942	13.218458
14.927637	1080.909576	13.223475
15.154428	1071.268525	13.228493
14.940438	1082.156031	13.233511
15.007645	1084.716807	13.238528
14.998421	1081.590214	13.243546
14.945747	1075.100026	13.248563
14.859700	1079.954239	13.253581
15.024284	1081.338001	13.258599
14.905765	1071.297796	13.263616
14.580887	1087.889163	13.268634
14.998510	1076.734248	13.273651
15.034241	1064.487339	13.278669
14.961375	1077.749037	13.283687
14.753404	1071.544214	13.288704
14.994011	1071.264024	13.293722
15.292930	1092.961937	13.298739
15.462866	1078.904169	13.303757
15.008017	1077.497098	13.308775
15.325249	1081.334928	13.313792
15.539060	1078.286319	13.318810
15.085212	1076.637785	13.323827
15.242689	1080.181698	13.328845
15.003793	1078.422457	13.333863
15.081258	1079.471365	13.338880
15.122842	1099.808711	13.343898
15.324526	1107.481820	13.348915
15.466821	1095.125559	13.353933
15.520725	1099.666642	13.358951
15.303955	1098.502753	13.363968
15.516002	1102.592479	13.368986
15.369682	1102.466571	13.374003
15.556169	1097.450863	13.379021
15.329408	1089.103542	13.384039
15.335162	1091.344315	13.389056
15.638981	1098.604940	13.394074
15.258369	1087.075723	13.399091
15.512305	1099.763246	13.404109
15.538149	1109.829578	13.409127
15.481812	1100.599016	13.414144
15.515243	1096.937212	13.419162
15.316917	1109.919132	13.424179
15.645157	1108.877737	13.429197
15.468387	1101.954285	13.434215
15.114146	1105.635714	13.439232
15.197759	1105.660554	13.444250
15.019330	1110.180301	13.449267
15.416876	1103.937198	13.454285
15.213274	1120.450201	13.459303
15.376010	1104.546178	13.464320
15.566439	1116.835521	13.469338
15.797639	1141.651054	13.474355
16.057295	1129.091446	13.479373
15.694951	1115.393315	13.484391
15.639927	1105.766735	13.489408
15.515221	1111.795454	13.494426
15.771870	1126.751357	13.499443
15.898393	1128.088371	13.504461
15.825513	1132.760337	13.509479
15.916564	1114.501229	13.514496
15.702826	1118.627669	13.519514
15.464835	1133.353761	13.524531
15.681606	1130.923740	13.529549
15.792975	1139.276836	13.534567
15.914128	1134.082181	13.539584
16.263059	1135.812289	13.544602
16.113383	1135.986884	13.549619
16.086436	1145.363066	13.554637
15.601558	1129.820920	13.559655
15.725901	1131.271857	13.564672
15.852630	1146.328370	13.569690
15.552208	1140.211817	13.574707
15.879451	1133.347554	13.579725
15.728384	1139.775259	13.584743
15.780876	1142.311709	13.589760
15.891271	1131.732735	13.594778
15.935782	1140.620217	13.599795
15.906572	1139.714256	13.604813
15.870018	1142.600799	13.609831
15.978402	1136.662513	13.614848
15.915344	1151.326057	13.619866
15.928416	1154.277223	13.624883
16.231810	1161.546608	13.629901
15.895988	1169.205838	13.634919
16.159701	1163.892748	13.639936
16.159194	1167.647404	13.644954
16.125082	1165.877436	13.649971
15.768085	1156.511913	13.654989
16.230515	1161.657731	13.660007
16.158769	1168.120559	13.665024
16.291994	1167.274353	13.670042
16.136586	1176.134668	13.675059
16.286406	1171.192110	13.680077
16.016250	1176.934904	13.685095
16.197956	1171.191934	13.690112
16.297859	1172.046030	13.695130
16.184403	1174.103105	13.700147
16.626561	1170.423828	13.705165
16.616306	1160.249748	13.710183
16.334120	1167.955025	13.715200
16.510973	1160.637730	13.720218
16.290058	1166.389899	13.725235
16.303511	1166.532223	13.730253
16.259314	1173.664404	13.735271
16.239082	1184.983467	13.740288
16.279948	1201.308543	13.745306
16.376005	1198.423933	13.750323
16.737405	1194.336806	13.755341
16.579644	1200.702661	13.760359
16.599290	1197.200074	13.765376
16.403690	1191.063817	13.770394
16.503703	1206.100791	13.775411
16.668164	1198.745178	13.780429
16.458804	1205.165814	13.785447
16.657426	1207.277602	13.790464
17.092115	1212.683687	13.795482
16.681003	1207.821614	13.800499
16.814489	1192.550774	13.805517
16.990261	1203.134229	13.810535
16.882397	1198.312778	13.815552
16.939249	1192.966749	13.820570
16.786849	1201.733093	13.825587
16.885245	1191.478251	13.830605
16.722261	1186.623990	13.835623
16.654003	1199.918195	13.840640
16.706617	1194.935207	13.845658
16.735670	1199.183722	13.850675
16.907052	1197.285515	13.855693
17.068892	1203.150400	13.860711
16.896562	1202.570990	13.865728
17.063052	1200.114629	13.870746
16.998196	1200.282293	13.875763
17.225149	1190.400236	13.880781
17.053252	1186.295553	13.885799
16.701049	1165.837572	13.890816
16.986794	1178.164943	13.895834
16.931791	1198.800815	13.900851
17.294179	1189.710612	13.905869
16.922354	1190.372436	13.910887
16.803614	1203.304575	13.915904
16.775004	1201.170762	13.920922
16.863694	1198.605821	13.925939
17.353670	1192.950654	13.930957
16.871910	1203.291453	13.935975
16.898824	1192.923051	13.940992
17.050922	1190.588143	13.946010
17.061504	1195.398673	13.951027
17.159998	1194.242903	13.956045
16.887661	1203.925377	13.961063
16.954223	1200.131619	13.966080
17.167432	1204.694921	13.971098
16.854695	1200.653069	13.976115
16.921547	1207.260305	13.981133
17.429398	1221.078510	13.986151
17.542717	1227.436579	13.991168
17.744701	1219.991107	13.996186
17.428012	1209.817249	14.001203
16.990953	1196.434494	14.006221
17.316744	1196.875929	14.011239
17.095047	1223.900341	14.016256
17.540540	1217.085779	14.021274
17.216601	1226.825803	14.026291
17.360818	1227.185848	14.031309
17.375774	1223.774763	14.036327
17.437548	1228.828573	14.041344
17.567973	1223.617004	14.046362
17.306799	1235.837003	14.051379
17.366475	1228.445945	14.056397
17.446436	1219.337252	14.061415
17.312995	1221.378151	14.066432
17.246123	1223.962880	14.071450
17.164056	1229.161898	14.076467
17.115207	1236.645608	14.081485
17.449756	1248.052913	14.086503
17.601670	1259.391015	14.091520
17.511179	1241.320394	14.096538
17.799503	1268.237767	14.101555
17.956323	1267.678554	14.106573
18.170663	1259.051487	14.111591
17.659642	1239.104615	14.116608
17.884526	1240.967815	14.121626
17.611571	1247.120874	14.126643
17.660451	1250.027368	14.131661
17.825273	1243.082828	14.136679
17.832959	1258.659239	14.141696
18.196611	1258.499635	14.146714
18.138492	1236.660890	14.151731
17.855986	1226.352260	14.156749
18.084909	1232.938430	14.161767
17.811038	1234.101504	14.166784
17.941169	1222.639427	14.171802
17.897325	1221.902586	14.176819
17.721085	1234.262852	14.181837
17.804091	1223.090801	14.186855
17.750411	1223.863212	14.191872
18.426746	1240.703487	14.196890
18.181152	1236.011264	14.201907
18.350031	1233.125634	14.206925
18.155752	1231.042616	14.211943
18.045348	1229.749347	14.216960
18.107391	1225.466842	14.221978
17.692215	1230.903558	14.226995
17.891822	1230.248904	14.232013
18.082752	1242.103689	14.237031
18.100974	1252.876771	14.242048
18.201170	1240.852594	14.247066
17.845312	1256.541240	14.252083
18.438510	1260.313336	14.257101
18.588697	1251.628775	14.262119
18.257387	1254.357784	14.267136
18.336097	1243.319477	14.272154
17.977521	1248.138676	14.277171
18.258846	1258.875171	14.282189
18.305774	1271.436147	14.287207
18.109508	1272.683036	14.292224
18.324452	1262.822010	14.297242
18.277677	1268.757609	14.302259
18.290690	1273.073353	14.307277
18.530007	1266.782526	14.312295
17.870328	1268.945037	14.317312
18.160866	1259.982594	14.322330
18.065681	1276.128691	14.327347
18.124307	1265.863642	14.332365
18.571357	1261.157126	14.337383
18.184975	1280.363267	14.342400
18.602241	1291.129476	14.347418
18.803672	1294.408932	14.352435
18.449863	1292.641988	14.357453
18.746878	1280.882450	14.362471
18.500227	1283.213086	14.367488
18.741986	1278.642049	14.372506
18.897853	1273.150318	14.377523
18.488659	1278.448486	14.382541
18.341928	1268.419309	14.387559
18.272811	1283.013913	14.392576
18.571867	1288.571553	14.397594
18.778635	1297.795049	14.402611
18.846567	1308.826449	14.407629
18.961789	1292.531525	14.412647
18.655188	1290.985679	14.417664
18.782325	1295.223129	14.422682
18.960782	1297.596685	14.427699
18.986822	1292.378725	14.432717
19.089754	1294.705322	14.437735
18.673906	1304.664095	14.442752
19.080673	1294.028749	14.447770
19.186734	1284.917278	14.452787
18.805333	1299.126567	14.457805
18.606539	1291.447537	14.462823
18.785888	1298.845935	14.467840
19.030907	1303.050522	14.472858
18.962580	1300.185383	14.477875
18.779549	1296.364552	14.482893
18.810349	1298.923508	14.487911
18.937783	1292.506302	14.492928
18.771117	1288.762677	14.497946
19.121461	1295.695089	14.502963
18.863352	1298.166181	14.507981
19.130178	1300.259821	14.512999
19.179342	1299.548543	14.518016
19.027081	1303.955181	14.523034
19.018381	1303.541215	14.528051
18.960136	1301.983258	14.533069
18.990572	1308.918552	14.538087
19.255969	1319.876388	14.543104
19.352070	1311.824255	14.548122
19.356647	1326.690535	14.553139
19.386387	1327.985499	14.558157
19.426771	1314.746537	14.563175
19.054512	1323.074752	14.568192
19.284288	1321.036782	14.573210
19.316566	1328.371127	14.578227
19.349541	1331.142884	14.583245
19.600180	1331.295807	14.588263
19.153752	1333.375651	14.593280
19.213277	1321.110337	14.598298
19.695697	1320.536678	14.603315
19.238579	1328.927731	14.608333
19.209317	1316.619425	14.613351
19.546139	1319.805066	14.618368
19.875175	1323.947357	14.623386
19.681096	1324.109414	14.628403
19.444263	1331.652774	14.633421
19.979840	1320.055129	14.638439
19.606065	1324.620604	14.643456
19.663842	1318.512490	14.648474
19.853473	1324.046895	14.653491
19.526021	1331.130502	14.658509
19.906295	1319.503610	14.663527
19.517802	1319.901700	14.668544
19.687520	1326.268990	14.673562
19.790949	1328.481158	14.678579
19.591639	1324.769687	14.683597
19.950874	1320.147930	14.688615
19.845639	1317.717166	14.693632
19.856653	1327.293845	14.698650
19.953964	1325.382867	14.703667
19.607844	1326.311272	14.708685
19.633801	1324.090090	14.713703
19.328919	1324.083479	14.718720
19.500099	1325.685725	14.723738
19.752731	1333.662881	14.728755
19.401724	1347.098807	14.733773
19.733183	1349.802345	14.738791
19.615635	1360.924464	14.743808
19.681624	1350.347168	14.748826
19.982626	1346.899609	14.753843
19.807070	1359.813911	14.758861
19.790016	1352.925359	14.763879
19.851804	1358.916073	14.768896
19.638717	1379.268516	14.773914
20.090050	1380.835886	14.778931
20.036227	1382.461347	14.783949
20.018199	1380.874101	14.788967
19.973250	1383.404454	14.793984
20.137690	1385.333558	14.799002
20.114651	1376.989908	14.804019
20.658937	1379.306365	14.809037
20.498998	1372.385127	14.814055
20.303604	1381.554287	14.819072
20.243501	1392.375641	14.824090
20.307910	1390.250244	14.829107
20.391025	1380.829172	14.834125
20.467168	1374.318849	14.839143
20.453762	1386.137642	14.844160
20.607420	1375.704871	14.849178
21.070159	1371.153972	14.854195
20.517079	1370.912830	14.859213
20.463209	1346.780273	14.864231
20.524161	1356.589232	14.869248
20.403288	1349.471420	14.874266
20.736280	1353.042681	14.879283
20.205423	1359.631258	14.884301
20.249176	1354.362325	14.889319
20.658977	1365.922808	14.894336
20.441418	1382.208118	14.899354
20.695084	1375.864097	14.904371
20.726513	1388.631636	14.909389
20.625852	1377.356775	14.914407
20.729589	1377.508585	14.919424
20.586776	1384.817570	14.924442
20.742664	1381.847656	14.929459
20.593565	1384.968754	14.934477
20.826687	1381.691240	14.939495
20.656198	1384.057132	14.944512
20.914439	1380.667412	14.949530
21.185736	1379.818649	14.954547
21.122653	1380.168868	14.959565
21.002137	1375.058945	14.964583
20.965724	1383.789889	14.969600
20.845870	1376.083600	14.974618
20.899637	1369.673813	14.979635
20.967660	1371.959347	14.984653
20.818393	1385.220650	14.989671
21.015661	1384.606134	14.994688
20.772904	1379.117850	14.999706
20.998846	1381.298758	15.004723
20.840691	1374.223507	15.009741
20.881112	1378.787467	15.014759
21.032152	1376.467666	15.019776
20.664019	1375.350420	15.024794
21.209252	1376.234263	15.029811
21.089246	1377.049725	15.034829
21.173142	1370.591067	15.039847
21.018551	1373.741216	15.044864
20.824563	1376.634925	15.049882
21.158833	1387.837885	15.054899
21.329809	1398.043191	15.059917
21.433262	1402.132443	15.064935
21.463935	1390.852991	15.069952
20.915011	1391.965876	15.074970
21.226871	1395.030875	15.079987
21.093445	1404.699769	15.085005
21.155227	1407.192608	15.090023
21.410938	1413.378820	15.095040
21.173162	1409.271187	15.100058
21.295890	1412.218845	15.105075
21.436182	1410.558195	15.110093
21.523762	1402.663699	15.115111
21.357432	1405.423335	15.120128
20.969051	1411.704769	15.125146
21.521617	1395.739960	15.130163
21.493725	1410.055668	15.135181
21.255632	1409.616429	15.140199
21.737659	1424.316906	15.145216
21.293679	1435.115128	15.150234
21.819044	1430.707974	15.155251
21.694369	1443.061657	15.160269
21.766105	1442.590898	15.165287
21.724302	1435.571183	15.170304
21.844221	1427.468604	15.175322
22.217605	1426.925951	15.180339
21.806238	1417.008905	15.185357
21.729790	1403.167812	15.190375
21.411594	1409.616950	15.195392
21.890909	1415.351116	15.200410
22.019714	1425.993266	15.205427
21.989702	1435.229207	15.210445
21.872576	1424.664013	15.215463
22.088069	1428.327534	15.220480
21.949671	1433.728815	15.225498
21.949094	1418.775138	15.230515
21.828970	1422.638587	15.235533
21.958967	1424.777491	15.240551
22.395362	1429.216392	15.245568
21.659999	1434.417356	15.250586
22.140717	1424.632759	15.255603
21.823117	1430.814131	15.260621
21.916706	1437.095835	15.265639
21.944048	1429.587012	15.270656
21.497165	1437.448755	15.275674
22.011073	1432.543962	15.280691
22.109310	1429.868759	15.285709
21.943116	1425.406824	15.290727
21.958696	1428.704032	15.295744
21.953544	1452.253220	15.300762
22.150693	1446.718981	15.305779
22.250169	1457.793102	15.310797
22.205773	1460.122422	15.315815
22.474490	1444.052918	15.320832
22.161124	1465.821446	15.325850
22.344692	1455.355139	15.330867
22.224939	1458.017336	15.335885
22.115430	1458.553549	15.340903
22.500606	1459.915750	15.345920
22.354288	1461.053825	15.350938
22.415173	1453.108604	15.355955
22.383278	1459.138064	15.360973
22.068587	1458.041897	15.365991
22.272901	1458.234952	15.371008
22.630884	1488.363950	15.376026
23.077443	1479.317730	15.381043
23.012241	1481.918759	15.386061
22.972212	1467.427196	15.391079
23.082105	1451.237103	15.396096
22.976017	1455.835927	15.401114
23.117945	1448.828947	15.406131
23.002316	1443.328291	15.411149
22.893153	1445.570885	15.416167
23.087420	1443.768457	15.421184
22.734189	1443.662372	15.426202
22.936820	1444.175933	15.431219
22.982727	1451.907828	15.436237
22.965906	1460.609597	15.441255
23.286076	1445.669019	15.446272
23.092032	1441.944839	15.451290
22.891030	1446.531790	15.456307
22.897546	1445.066841	15.461325
22.768664	1451.037533	15.466343
22.733177	1442.738811	15.471360
22.705972	1451.228740	15.476378
22.895502	1447.036112	15.481395
22.843039	1455.211563	15.486413
22.806163	1446.146845	15.491431
23.145520	1456.663880	15.496448
22.865703	1450.879377	15.501466
23.050356	1447.060138	15.506483
22.836330	1460.858113	15.511501
22.675222	1472.285695	15.516519
23.318557	1473.464705	15.521536
23.240863	1486.382425	15.526554
23.472243	1487.662581	15.531571
23.367009	1483.314551	15.536589
23.287354	1494.739318	15.541607
23.709036	1484.802849	15.546624
23.172030	1488.575389	15.551642
23.373376	1483.062881	15.556659
23.151809	1491.702257	15.561677
22.914992	1493.793145	15.566695
23.310734	1483.295101	15.571712
23.106996	1483.098572	15.576730
23.125263	1485.513982	15.581747
23.636599	1482.600251	15.586765
23.285623	1488.643679	15.591783
23.676407	1490.124231	15.596800
23.482591	1497.853645	15.601818
23.762735	1502.104247	15.606835
23.792632	1490.405030	15.611853
23.311606	1489.721529	15.616871
23.504656	1496.779224	15.621888
23.437023	1507.846750	15.626906
23.615218	1509.349643	15.631923
23.602581	1504.377535	15.636941
23.671124	1519.907938	15.641959
24.107965	1501.991365	15.646976
23.939166	1505.298985	15.651994
24.156289	1511.600653	15.657011
23.970289	1507.805256	15.662029
23.862755	1504.389946	15.667047
23.982282	1499.116118	15.672064
23.980467	1505.171919	15.677082
23.905898	1503.788071	15.682099
24.040067	1494.825549	15.687117
23.875356	1504.696104	15.692135
24.252091	1502.591508	15.697152
23.961482	1496.571208	15.702170
24.102826	1499.697276	15.707187
24.232984	1506.379993	15.712205
23.968420	1505.224561	15.717223
24.129163	1493.946567	15.722240
24.121961	1497.003103	15.727258
24.159204	1507.659063	15.732275
24.462647	1501.482330	15.737293
24.310023	1497.183067	15.742311
24.313152	1499.256346	15.747328
24.253436	1511.722560	15.752346
24.423027	1497.562613	15.757363
24.367814	1491.724640	15.762381
24.244154	1503.176368	15.767399
24.198214	1500.189792	15.772416
24.126509	1501.164970	15.777434
23.975052	1507.534830	15.782451
24.312139	1509.378143	15.787469
24.169018	1537.558650	15.792487
24.257217	1535.106710	15.797504
24.142500	1540.979047	15.802522
24.489452	1533.616145	15.807539
24.609045	1537.490001	15.812557
24.303620	1547.540901	15.817575
24.762989	1527.064838	15.822592
24.669651	1539.130980	15.827610
24.480190	1537.070742	15.832627
24.572843	1538.712953	15.837645
24.510361	1547.715975	15.842663
24.828642	1533.408803	15.847680
24.661808	1530.549862	15.852698
24.267840	1537.951401	15.857715
24.513352	1550.985424	15.862733
24.771459	1568.217964	15.867751
25.464339	1560.989980	15.872768
25.253864	1558.877905	15.877786
25.147035	1550.566509	15.882803
25.047921	1522.593079	15.887821
24.838215	1529.840560	15.892839
25.150897	1525.612207	15.897856
24.973118	1523.710647	15.902874
24.899963	1531.664985	15.907891
24.931247	1527.432354	15.912909
24.767707	1550.196566	15.917927
25.371937	1550.364473	15.922944
25.245345	1555.414092	15.927962
25.431802	1553.648764	15.932979
25.446820	1549.189125	15.937997
25.179813	1536.425121	15.943015
25.672465	1528.665165	15.948032
25.304793	1530.660769	15.953050
25.138653	1520.053223	15.958067
25.445216	1518.718183	15.963085
25.208279	1526.087271	15.968103
25.378096	1513.179848	15.973120
25.358695	1516.860951	15.978138
25.141507	1525.240408	15.983155
25.561231	1536.773203	15.988173
25.287883	1543.821395	15.993191
25.519484	1543.495055	15.998208
25.425458	1544.485537	16.003226
25.240033	1553.530531	16.008243
25.463476	1549.301567	16.013261
25.499246	1550.708922	16.018279
25.503990	1549.058062	16.023296
25.579334	1550.140616	16.028314
25.695546	1550.527931	16.033331
25.786489	1543.600780	16.038349
25.702128	1545.572005	16.043367
25.663448	1540.833881	16.048384
25.798645	1542.752092	16.053402
25.611146	1553.664288	16.058419
25.564040	1548.617362	16.063437
25.374731	1561.314845	16.068455
25.752035	1567.281643	16.073472
25.791005	1567.348700	16.078490
25.935304	1586.409853	16.083507
26.439106	1587.271428	16.088525
25.950327	1579.507517	16.093543
26.139742	1563.376006	16.098560
25.861945	1560.263192	16.103578
26.317612	1561.346862	16.108595
26.069346	1542.189717	16.113613
25.674666	1559.912552	16.118631
25.819693	1562.880961	16.123648
25.782386	1571.052001	16.128666
25.850899	1585.353121	16.133683
26.219926	1571.654173	16.138701
26.102954	1576.157797	16.143719
26.043259	1586.997329	16.148736
26.104266	1578.867797	16.153754
26.156851	1583.818730	16.158771
26.438675	1581.383204	16.163789
26.192940	1578.482576	16.168807
26.575076	1580.000978	16.173824
26.489619	1587.140169	16.178842
26.411181	1584.602587	16.183859
26.565706	1574.776145	16.188877
26.404207	1585.197718	16.193895
26.637348	1573.610302	16.198912
26.805751	1582.939902	16.203930
26.500402	1584.895691	16.208947
26.709733	1576.540102	16.213965
26.342127	1573.648003	16.218983
26.306292	1577.674309	16.224000
26.515450	1581.697131	16.229018
26.482636	1596.453331	16.234035
26.838034	1603.405517	16.239053
26.894091	1603.095983	16.244071
26.712168	1600.773110	16.249088
27.065160	1610.735319	16.254106
26.728121	1592.780215	16.259123
26.841794	1583.942076	16.264141
27.219499	1602.062637	16.269159
27.323383	1579.673871	16.274176
27.163296	1563.718998	16.279194
26.696622	1571.888761	16.284211
26.643000	1565.872177	16.289229
26.873123	1572.890911	16.294247
26.971785	1585.839208	16.299264
27.299882	1591.426014	16.304282
27.233963	1584.588734	16.309299
27.393201	1573.045024	16.314317
27.224142	1564.942104	16.319335
27.234474	1563.117902	16.324352
27.237252	1560.300010	16.329370
27.250022	1566.900002	16.334387
27.138358	1560.489525	16.339405
27.039437	1565.706007	16.344423
27.302782	1567.355047	16.349440
27.238921	1574.618992	16.354458
27.070984	1586.822088	16.359475
27.294855	1587.049507	16.364493
27.276214	1595.000379	16.369511
26.989358	1586.476229	16.374528
27.570413	1587.967270	16.379546
27.149835	1598.683206	16.384563
27.302329	1578.540820	16.389581
27.637388	1591.120574	16.394599
27.343681	1598.077483	16.399616
27.232537	1586.415869	16.404634
27.369746	1603.464323	16.409651
27.570547	1607.396223	16.414669
27.604675	1621.496198	16.419687
27.677017	1621.387094	16.424704
27.954071	1626.502887	16.429722
27.701589	1616.281342	16.434739
27.803810	1628.621887	16.439757
27.791952	1623.743694	16.444775
27.771890	1622.366966	16.449792
27.871262	1621.485982	16.454810
27.626592	1624.302494	16.459827
28.024595	1615.816506	16.464845
28.064282	1616.711873	16.469863
27.778609	1629.990811	16.474880
28.272150	1629.187186	16.479898
28.246545	1628.874615	16.484915
27.830987	1616.036288	16.489933
28.016950	1625.867076	16.494951
27.936794	1626.568893	16.499968
28.265334	1619.687668	16.504986
27.945332	1612.271584	16.510003
28.114670	1614.444559	16.515021
28.388851	1619.768866	16.520039
28.216386	1623.841185	16.525056
28.081247	1623.659888	16.530074
27.836588	1625.821370	16.535091
28.266826	1619.838961	16.540109
28.206802	1626.392551	16.545127
28.069239	1622.548772	16.550144
28.513139	1629.351324	16.555162
28.464123	1652.710653	16.560179
28.612345	1640.957324	16.565197
28.490225	1631.572770	16.570215
28.567602	1636.590873	16.575232
28.528964	1630.193886	16.580250
28.281137	1631.733537	16.585267
28.645083	1639.453120	16.590285
28.833260	1664.109307	16.595303
28.564057	1658.172992	16.600320
28.829635	1644.959515	16.605338
28.834828	1658.574806	16.610355
28.856138	1640.436034	16.615373
28.853688	1645.220909	16.620391
28.645659	1638.440353	16.625408
28.934882	1638.513686	16.630426
28.947986	1653.217870	16.635443
29.118959	1641.435390	16.640461
29.053268	1629.467060	16.645479
28.698511	1618.899473	16.650496
29.099800	1629.675647	16.655514
28.618041	1641.559832	16.660531
28.623009	1645.310354	16.665549
28.908334	1653.840270	16.670567
28.969981	1660.689473	16.675584
29.045578	1646.400650	16.680602
28.521118	1652.505484	16.685619
29.274589	1657.138673	16.690637
29.055984	1647.885983	16.695655
28.963267	1642.424377	16.700672
29.184595	1649.060597	16.705690
28.997002	1662.021623	16.710707
29.044822	1673.874608	16.715725
29.281731	1678.908285	16.720743
28.979582	1677.285492	16.725760
29.266243	1689.214160	16.730778
29.447299	1687.028703	16.735795
29.274931	1686.488252	16.740813
29.170271	1686.366476	16.745831
29.389871	1686.373569	16.750848
29.717321	1685.294674	16.755866
29.273041	1686.631001	16.760883
29.413221	1684.510756	16.765901
29.788437	1685.682328	16.770919
29.635863	1697.565692	16.775936
30.063645	1689.252869	16.780954
29.613468	1696.332911	16.785971
29.659317	1684.065041	16.790989
30.019906	1693.686133	16.796007
29.747225	1689.508415	16.801024
29.815006	1690.252116	16.806042
29.833385	1699.515647	16.811059
29.956547	1696.711887	16.816077
30.661206	1703.240701	16.821095
30.153812	1699.106295	16.826112
30.176951	1678.196875	16.831130
30.296916	1679.600563	16.836147
30.391409	1683.242808	16.841165
30.487888	1677.178347	16.846183
29.921621	1679.651021	16.851200
30.210567	1679.827732	16.856218
29.869094	1681.976682	16.861235
29.922704	1676.126561	16.866253
30.286605	1672.440024	16.871271
29.895209	1684.215227	16.876288
30.091673	1670.166413	16.881306
30.137596	1675.327110	16.886323
30.236988	1684.303461	16.891341
30.507426	1672.022104	16.896359
30.122552	1678.061760	16.901376
30.586988	1700.637389	16.906394
30.192733	1689.635591	16.911411
30.303999	1707.409414	16.916429
30.263323	1714.304287	16.921447
29.941232	1708.452864	16.926464
30.311250	1695.815903	16.931482
30.096899	1701.162515	16.936499
30.422008	1708.735225	16.941517
30.364348	1702.138426	16.946535
30.421439	1721.949297	16.951552
30.996573	1720.629298	16.956570
31.218357	1728.810551	16.961587
31.125588	1719.281741	16.966605
31.081208	1706.912834	16.971623
31.177103	1703.967141	16.976640
31.157435	1699.122494	16.981658
30.622653	1702.041483	16.986675
30.693002	1695.068265	16.991693
30.740795	1694.844926	16.996711
30.586696	1707.442432	17.001728
30.913150	1718.080858	17.006746
30.791988	1736.262368	17.011763
31.229317	1734.536457	17.016781
31.252219	1726.103737	17.021799
31.071846	1736.413585	17.026816
31.112068	1734.267141	17.031834
31.147553	1734.195226	17.036851
31.197270	1726.592021	17.041869
31.407321	1725.762416	17.046887
31.113577	1735.636334	17.051904
31.383160	1722.421539	17.056922
31.391176	1733.035248	17.061939
31.186113	1735.149656	17.066957
31.108225	1725.077903	17.071975
31.319706	1728.778965	17.076992
31.208054	1725.854379	17.082010
31.228539	1728.418654	17.087027
31.795453	1744.979772	17.092045
31.788337	1729.727109	17.097063
31.634147	1740.866580	17.102080
31.466528	1730.257755	17.107098
31.621334	1728.622031	17.112115
31.794110	1746.002517	17.117133
31.514545	1747.467514	17.122151
31.300204	1753.754178	17.127168
31.688276	1752.355852	17.132186
31.658448	1757.483431	17.137203
31.456453	1753.673689	17.142221
31.792529	1743.358143	17.147239
31.593498	1757.381631	17.152256
31.454764	1755.308060	17.157274
31.632676	1764.267545	17.162291
31.806360	1784.736505	17.167309
31.917208	1777.951019	17.172327
31.941391	1778.421257	17.177344
32.029898	1779.653208	17.182362
32.349766	1773.486840	17.187379
32.284588	1771.263136	17.192397
32.648728	1779.021532	17.197415
32.466053	1780.698443	17.202432
32.775569	1787.028652	17.207450
32.829177	1787.880592	17.212467
32.568963	1765.444457	17.217485
32.562447	1747.051136	17.222503
32.388293	1750.807075	17.227520
32.437822	1727.224674	17.232538
32.354507	1741.637437	17.237555
32.462229	1748.837286	17.242573
32.602629	1735.546596	17.247591
32.348953	1737.966047	17.252608
32.313213	1734.192606	17.257626
32.448520	1756.362532	17.262643
32.665328	1771.767520	17.267661
32.786214	1768.589761	17.272679
32.432557	1779.623658	17.277696
32.677015	1784.706115	17.282714
32.769488	1781.207304	17.287731
32.845511	1787.004911	17.292749
33.207844	1771.032969	17.297767
32.771674	1776.012379	17.302784
32.880060	1768.811215	17.307802
32.953878	1776.355810	17.312819
32.664028	1778.730661	17.317837
32.609604	1772.332287	17.322855
32.841497	1773.810980	17.327872
32.805320	1766.872456	17.332890
32.823875	1774.275415	17.337907
32.839416	1784.649167	17.342925
33.230636	1795.069292	17.347943
33.292617	1805.559974	17.352960
33.048824	1803.846235	17.357978
33.235842	1799.651172	17.362995
33.202694	1802.155039	17.368013
33.357218	1809.560542	17.373031
32.979089	1813.022883	17.378048
33.415471	1808.275255	17.383066
33.798052	1804.681061	17.388083
33.447143	1807.401003	17.393101
33.638385	1810.837551	17.398119
33.447348	1802.221077	17.403136
33.456521	1796.730965	17.408154
33.732273	1802.558162	17.413171
33.509568	1804.929006	17.418189
33.462180	1799.988330	17.423207
33.273374	1796.602132	17.428224
33.341122	1798.036308	17.433242
33.378091	1812.618015	17.438259
33.629945	1838.069565	17.443277
34.008700	1837.721461	17.448295
33.633195	1830.827570	17.453312
34.011675	1833.766505	17.458330
33.889011	1830.301857	17.463347
33.891262	1838.489531	17.468365
34.076050	1822.683867	17.473383
34.440955	1831.841595	17.478400
33.899774	1827.537168	17.483418
34.262474	1831.422688	17.488435
34.173272	1829.561564	17.493453
34.515205	1808.785086	17.498471
34.115495	1828.677883	17.503488
34.192467	1824.427780	17.508506
34.802423	1824.901401	17.513523
34.201780	1825.539062	17.518541
34.568309	1822.667506	17.523559
34.206931	1820.838370	17.528576
34.066434	1827.172893	17.533594
34.554083	1820.973268	17.538611
34.309366	1823.845525	17.543629
34.304385	1821.304424	17.548647
34.688186	1813.631795	17.553664
34.680726	1815.164414	17.558682
34.703131	1816.734220	17.563699
34.305953	1813.335607	17.568717
34.328879	1817.304830	17.573735
34.472914	1819.875077	17.578752
34.346035	1820.564744	17.583770
34.471006	1810.561957	17.588787
33.971156	1826.552107	17.593805
34.297585	1832.455773	17.598823
34.279693	1842.140686	17.603840
34.296912	1849.972392	17.608858
34.673300	1852.893569	17.613875
34.946171	1871.699211	17.618893
35.248119	1878.021654	17.623911
35.189309	1886.557985	17.628928
34.924079	1874.905279	17.633946
35.441652	1870.250108	17.638963
35.253941	1875.089092	17.643981
35.475200	1852.820083	17.648999
35.325679	1847.950790	17.654016
35.261872	1840.141711	17.659034
35.400353	1842.516841	17.664051
35.209829	1845.877132	17.669069
35.336064	1837.466837	17.674087
35.127826	1845.342885	17.679104
35.514376	1860.615002	17.684122
35.552279	1848.906514	17.689139
35.472366	1871.240699	17.694157
35.564018	1865.158656	17.699175
35.497798	1871.210286	17.704192
35.590903	1878.235073	17.709210
35.977826	1861.053215	17.714227
35.748610	1869.139606	17.719245
35.800263	1860.835706	17.724263
35.896883	1856.158383	17.729280
35.715726	1882.637157	17.734298
35.955176	1859.916367	17.739315
35.957765	1858.342592	17.744333
36.151298	1858.949787	17.749351
36.027706	1847.641760	17.754368
35.472382	1851.684310	17.759386
35.961239	1843.021589	17.764403
35.586771	1864.529156	17.769421
35.700011	1868.154175	17.774439
35.821119	1870.065111	17.779456
35.886452	1863.359739	17.784474
36.045882	1863.016584	17.789491
35.588634	1864.202724	17.794509
36.044702	1873.010807	17.799527
36.161602	1885.443216	17.804544
36.031885	1892.344222	17.809562
36.478780	1891.771890	17.814579
36.402073	1895.533018	17.819597
36.305826	1890.311642	17.824615
36.369871	1888.108884	17.829632
36.282616	1888.717212	17.834650
36.523918	1881.370031	17.839667
35.934404	1886.185272	17.844685
36.168839	1892.111250	17.849703
36.437828	1901.175238	17.854720
36.442243	1910.229614	17.859738
36.816784	1911.491659	17.864755
36.491338	1920.908981	17.869773
36.685169	1909.903726	17.874791
37.080306	1920.144374	17.879808
36.861807	1916.773882	17.884826
37.039968	1911.013312	17.889843
37.169650	1918.751083	17.894861
37.092262	1900.582257	17.899879
37.211626	1900.989531	17.904896
36.855639	1916.178139	17.909914
36.979355	1903.613992	17.914931
37.135497	1909.848352	17.919949
37.082638	1897.249225	17.924967
37.249444	1900.403054	17.929984
36.787888	1912.576396	17.935002
37.192629	1897.102767	17.940019
37.208607	1903.307341	17.945037
36.926347	1919.366930	17.950055
37.022405	1896.405641	17.955072
37.101773	1902.879627	17.960090
37.408246	1908.730131	17.965107
37.008064	1912.425442	17.970125
37.395747	1925.668348	17.975143
37.575742	1926.379149	17.980160
37.242882	1941.607262	17.985178
37.691409	1937.609468	17.990195
37.681283	1944.139004	17.995213
37.886475	1935.376670	18.000231
37.714205	1935.949055	18.005248
37.419224	1930.779206	18.010266
37.951284	1925.552991	18.015283
38.216939	1928.190746	18.020301
37.758149	1925.645892	18.025319
38.048778	1928.396238	18.030336
37.675851	1934.804054	18.035354
38.202243	1917.119417	18.040371
38.003064	1931.674718	18.045389
38.003738	1931.725864	18.050407
38.155492	1924.838880	18.055424
38.009591	1917.669829	18.060442
38.115338	1923.083487	18.065459
38.093410	1921.025035	18.070477
38.143516	1927.184810	18.075495
37.992039	1921.767456	18.080512
37.966943	1931.524474	18.085530
38.417044	1946.832430	18.090547
38.485488	1959.970463	18.095565
38.543138	1953.745400	18.100583
38.527616	1959.201943	18.105600
38.462509	1955.910804	18.110618
38.809834	1958.868101	18.115635
38.624708	1964.249142	18.120653
38.390515	1962.648549	18.125671
38.693423	1948.391756	18.130688
38.696553	1960.668243	18.135706
39.209146	1948.587173	18.140723
39.155949	1951.487836	18.145741
38.969207	1958.679169	18.150759
39.199679	1956.263881	18.155776
38.722722	1949.985647	18.160794
38.859641	1942.613172	18.165811
38.540809	1953.804213	18.170829
38.603749	1966.034802	18.175847
38.816706	1952.205421	18.180864
38.739478	1967.917435	18.185882
38.773061	1950.955858	18.190899
38.877394	1948.626369	18.195917
39.017935	1965.745729	18.200935
38.688360	1973.758219	18.205952
39.093674	1989.953636	18.210970
38.996991	1988.261426	18.215987
38.967070	1984.916834	18.221005
39.013221	1996.433964	18.226023
39.091660	1993.471812	18.231040
39.208109	2012.012563	18.236058
39.403448	2008.294362	18.241075
39.197412	2018.567502	18.246093
39.467467	2022.196955	18.251111
39.819069	2018.040178	18.256128
39.536777	2007.031262	18.261146
39.778550	2022.258379	18.266163
40.120212	2024.553509	18.271181
40.125090	2006.754582	18.276199
40.261667	2012.020870	18.281216
40.199352	2015.341705	18.286234
40.124565	2001.521057	18.291251
40.006265	1983.146911	18.296269
39.623929	1978.291841	18.301287
39.697763	1982.625682	18.306304
39.761585	2003.406362	18.311322
39.938910	2002.745321	18.316339
40.102447	2005.435198	18.321357
40.336848	2011.102201	18.326375
40.396901	1997.410044	18.331392
40.148885	2010.691352	18.336410
40.127141	2006.438026	18.341427
40.123519	2000.562007	18.346445
40.012135	2004.238745	18.351463
40.270207	2000.193679	18.356480
40.199364	1998.895183	18.361498
40.572450	2003.967086	18.366515
40.565499	2016.529504	18.371533
40.425571	2021.676153	18.376551
40.877734	2020.792548	18.381568
40.714331	2034.398438	18.386586
40.716806	2019.602120	18.391603
40.918166	2023.348426	18.396621
40.855965	2024.263804	18.401639
40.807898	2023.218404	18.406656
40.828709	2034.220123	18.411674
41.016351	2020.162214	18.416691
41.121912	2026.179809	18.421709
40.743834	2033.365988	18.426727
41.020482	2023.819441	18.431744
41.085530	2028.072865	18.436762
41.109517	2017.998650	18.441779
41.184538	2015.751939	18.446797
40.991246	2030.631718	18.451815
41.127539	2022.615285	18.456832
41.067186	2019.135770	18.461850
41.235012	2034.146011	18.466867
41.459412	2015.102860	18.471885
41.240430	2013.093691	18.476903
41.565998	2010.754401	18.481920
41.240640	2012.051615	18.486938
41.206003	2021.912026	18.491955
41.085424	2022.616801	18.496973
41.118109	2041.142890	18.501991
41.602164	2044.565153	18.507008
41.641913	2056.851805	18.512026
41.456275	2058.219230	18.517043
41.697923	2043.980346	18.522061
41.725937	2057.463886	18.527079
42.271892	2052.892347	18.532096
41.829145	2054.725048	18.537114
41.785864	2041.645139	18.542131
42.011209	2056.890555	18.547149
42.234432	2046.649356	18.552167
42.357350	2043.592058	18.557184
42.041696	2039.751426	18.562202
42.068182	2039.605021	18.567219
42.125082	2046.955519	18.572237
41.685446	2056.194965	18.577255
42.301823	2048.255661	18.582272
42.218586	2048.831641	18.587290
42.012890	2048.058128	18.592307
42.477519	2050.937402	18.597325
41.938721	2071.050324	18.602343
42.497341	2073.761331	18.607360
42.214071	2069.968877	18.612378
42.312301	2081.991976	18.617395
42.873453	2077.999549	18.622413
42.391685	2076.761868	18.627431
42.801945	2074.633746	18.632448
42.782736	2069.090359	18.637466
42.987689	2068.035029	18.642483
42.802930	2064.879376	18.647501
42.452354	2070.895014	18.652519
42.858249	2066.450936	18.657536
43.287312	2063.261752	18.662554
42.824781	2075.612331	18.667571
42.863548	2068.339866	18.672589
42.917606	2072.022740	18.677607
43.014107	2066.574197	18.682624
43.031937	2059.130411	18.687642
43.031320	2058.906210	18.692659
42.991208	2056.331707	18.697677
42.961622	2089.155959	18.702695
43.344929	2088.001279	18.707712
43.415084	2092.810118	18.712730
43.132202	2098.952360	18.717747
43.765700	2094.742286	18.722765
43.465969	2099.303230	18.727783
43.426652	2096.799841	18.732800
43.512300	2107.475970	18.737818
43.510459	2099.856891	18.742835
43.641438	2092.560121	18.747853
43.477060	2105.406277	18.752871
43.460764	2098.002557	18.757888
43.315569	2095.179300	18.762906
43.523298	2103.949824	18.767923
43.922400	2109.483358	18.772941
43.775248	2129.397593	18.777959
43.881795	2131.372970	18.782976
44.346004	2124.372261	18.787994
44.047966	2132.744740	18.793011
44.081387	2114.276869	18.798029
43.934940	2132.006182	18.803047
44.182283	2124.930496	18.808064
44.165120	2128.726521	18.813082
43.946272	2124.754921	18.818099
44.380444	2122.760622	18.823117
44.414939	2121.641341	18.828135
44.485566	2122.546585	18.833152
44.623450	2123.764695	18.838170
44.173169	2124.725316	18.843187
44.216782	2119.198693	18.848205
44.089861	2121.537025	18.853223
44.111345	2131.998405	18.858240
44.425660	2134.758063	18.863258
44.492533	2154.427338	18.868275
44.767030	2146.077207	18.873293
44.695169	2157.639744	18.878311
45.208377	2155.974470	18.883328
45.151789	2142.004050	18.888346
44.894587	2150.215869	18.893363
44.910716	2147.424007	18.898381
44.793507	2162.472620	18.903399
45.357745	2152.859572	18.908416
44.898773	2144.341114	18.913434
44.940386	2148.861607	18.918451
45.361711	2140.661213	18.923469
45.155886	2151.720545	18.928487
44.943683	2148.361558	18.933504
45.256673	2138.140893	18.938522
45.089517	2149.931946	18.943539
45.097541	2150.170441	18.948557
45.302370	2165.252049	18.953575
45.191587	2163.070271	18.958592
45.583535	2178.173720	18.963610
45.205132	2185.677314	18.968627
45.563426	2167.731814	18.973645
45.135732	2177.202996	18.978663
45.443926	2174.728575	18.983680
45.558448	2168.767424	18.988698
45.640312	2192.036658	18.993715
45.733624	2200.191760	18.998733
46.103374	2203.640624	19.003751
46.698945	2193.602730	19.008768
46.643846	2179.608607	19.013786
46.259172	2166.630279	19.018803
46.618789	2163.905851	19.023821
46.250251	2166.028436	19.028839
46.250686	2172.502195	19.033856
46.426691	2152.802373	19.038874
46.253695	2160.362552	19.043891
46.589921	2166.607214	19.048909
46.566809	2160.439110	19.053927
46.824525	2158.542857	19.058944
46.952827	2152.596165	19.063962
46.775247	2156.256715	19.068979
46.498022	2130.856824	19.073997
46.481147	2134.215644	19.079015
45.982122	2152.093591	19.084032
46.543659	2147.852879	19.089050
46.312481	2162.558159	19.094067
46.550024	2167.785377	19.099085
46.487247	2165.741712	19.104103
46.291991	2156.320307	19.109120
46.585523	2171.278613	19.114138
46.613309	2182.876468	19.119155
46.889663	2188.302770	19.124173
46.888274	2194.829787	19.129191
46.641292	2194.887809	19.134208
47.011618	2190.609400	19.139226
46.917283	2201.138978	19.144243
47.001010	2202.928981	19.149261
46.826224	2225.480911	19.154279
46.893195	2228.099982	19.159296
47.289198	2230.366678	19.164314
46.841897	2229.511636	19.169331
47.128318	2228.455430	19.174349
47.400453	2240.594978	19.179367
47.464316	2254.300893	19.184384
47.806363	2250.773329	19.189402
47.656418	2256.416349	19.194419
47.637242	2254.969149	19.199437
47.750904	2258.766616	19.204455
47.964344	2251.716946	19.209472
48.134117	2253.422269	19.214490
47.930043	2258.791585	19.219507
48.258447	2262.540574	19.224525
48.282890	2243.163686	19.229543
48.125104	2247.929738	19.234560
48.323902	2244.408133	19.239578
48.394042	2251.157386	19.244595
48.530140	2248.230141	19.249613
48.118322	2230.605318	19.254631
48.211003	2227.439803	19.259648
48.330846	2221.712966	19.264666
48.498476	2251.062594	19.269683
48.344216	2226.884624	19.274701
48.528573	2234.240130	19.279719
48.416767	2246.203588	19.284736
48.525132	2250.053104	19.289754
48.386155	2237.003211	19.294771
48.544792	2244.259636	19.299789
48.932872	2251.998767	19.304807
48.515056	2240.749309	19.309824
48.916413	2241.926251	19.314842
48.682747	2242.375734	19.319859
48.682656	2236.252020	19.324877
48.647775	2243.131015	19.329895
48.593533	2252.076990	19.334912
48.762632	2239.015157	19.339930
48.739718	2243.073356	19.344947
49.374626	2247.759980	19.349965
49.254884	2266.963042	19.354983
49.068290	2275.986408	19.360000
49.147198	2268.493062	19.365018
49.055648	2269.380434	19.370035
49.349682	2271.944668	19.375053
49.313337	2265.413783	19.380071
49.163847	2274.830980	19.385088
49.268605	2264.212795	19.390106
49.110667	2268.408656	19.395123
49.294353	2277.580459	19.400141
49.321737	2289.469969	19.405159
49.312614	2298.145547	19.410176
49.611821	2287.132058	19.415194
49.488595	2301.725938	19.420211
49.731777	2296.023174	19.425229
49.979998	2295.603532	19.430247
49.800546	2306.083080	19.435264
50.238284	2297.751360	19.440282
50.215309	2316.732212	19.445299
50.477392	2312.373636	19.450317
50.134673	2298.167510	19.455335
50.129889	2289.106637	19.460352
50.041126	2302.354791	19.465370
50.037821	2312.422199	19.470387
50.345392	2314.732652	19.475405
50.460601	2309.169918	19.480423
49.931067	2306.118234	19.485440
50.301010	2311.202175	19.490458
50.044332	2312.867949	19.495475
50.302240	2318.503429	19.500493
51.055743	2337.747490	19.505511
50.670852	2347.409124	19.510528
51.123418	2327.778327	19.515546
51.022292	2337.750115	19.520563
50.898698	2324.673396	19.525581
51.065421	2319.839873	19.530599
50.758420	2331.250078	19.535616
51.136390	2338.208711	19.540634
51.203549	2329.542777	19.545651
51.203875	2333.151137	19.550669
51.120601	2339.198091	19.555687
51.264212	2341.795857	19.560704
51.518839	2320.828808	19.565722
51.579057	2340.538786	19.570739
51.150799	2347.971374	19.575757
51.510049	2331.785603	19.580775
51.437257	2330.241952	19.585792
51.736180	2332.103484	19.590810
51.096727	2332.608809	19.595827
51.315820	2334.063887	19.600845
51.526767	2335.901773	19.605863
51.529691	2335.415393	19.610880
51.764394	2329.169187	19.615898
51.789587	2336.882510	19.620915
51.792037	2328.502639	19.625933
51.598227	2324.374895	19.630951
51.445991	2334.919643	19.635968
51.733428	2347.166777	19.640986
51.856603	2349.630531	19.646003
51.887855	2355.021813	19.651021
51.947408	2356.125536	19.656039
51.973661	2360.799797	19.661056
52.294881	2350.567004	19.666074
51.843033	2359.771446	19.671091
52.181226	2378.839724	19.676109
52.468973	2382.167350	19.681127
52.619164	2397.601689	19.686144
52.532428	2383.058130	19.691162
52.633957	2395.355314	19.696179
52.513281	2391.889029	19.701197
52.826944	2377.639119	19.706215
52.909810	2381.216134	19.711232
53.227315	2379.008230	19.716250
53.172517	2376.513455	19.721267
52.760382	2372.108813	19.726285
52.816902	2365.370234	19.731303
52.930249	2373.317411	19.736320
53.269645	2370.950982	19.741338
53.145880	2376.310413	19.746355
52.888991	2382.276242	19.751373
53.101232	2358.075883	19.756391
52.792770	2372.651823	19.761408
52.948690	2362.023148	19.766426
53.183413	2389.556800	19.771443
53.369015	2403.167539	19.776461
53.813126	2399.228228	19.781479
53.574656	2405.670311	19.786496
53.785203	2412.105512	19.791514
53.572760	2406.703180	19.796531
53.384335	2405.416995	19.801549
53.689365	2400.422217	19.806567
53.341217	2405.594939	19.811584
53.498011	2408.314345	19.816602
53.642178	2409.752681	19.821619
53.707076	2433.857098	19.826637
54.160803	2434.325658	19.831655
53.669491	2430.755274	19.836672
54.017237	2434.558782	19.841690
53.743294	2423.143300	19.846707
53.936934	2442.119807	19.851725
54.193423	2445.607914	19.856743
54.527570	2456.780183	19.861760
54.721733	2463.164377	19.866778
54.745764	2456.372471	19.871795
54.600864	2445.431669	19.876813
54.802383	2425.360582	19.881831
54.518914	2434.595900	19.886848
54.960470	2434.692093	19.891866
54.972363	2434.968336	19.896883
54.468319	2435.376293	19.901901
54.715597	2450.268504	19.906919
54.850893	2449.839963	19.911936
55.220370	2455.806830	19.916954
55.377761	2471.020189	19.921971
55.323272	2450.354420	19.926989
55.437810	2428.272677	19.932007
54.796332	2431.185613	19.937024
55.224936	2440.061746	19.942042
55.104165	2439.766852	19.947059
54.942251	2450.937439	19.952077
55.420262	2453.209906	19.957095
54.935618	2457.552516	19.962112
55.414376	2448.805703	19.967130
55.698622	2457.606892	19.972147
55.196618	2456.036133	19.977165
55.122767	2444.453132	19.982183
54.950707	2463.819598	19.987200
55.427014	2472.024536	19.992218
55.798130	2476.147197	19.997235
55.648387	2484.981540	20.002253
56.059284	2475.239119	20.007271
55.759314	2481.404609	20.012288
55.652631	2483.525889	20.017306
55.802616	2483.009888	20.022323
55.695667	2509.136752	20.027341
55.844330	2506.954172	20.032359
56.103040	2511.547154	20.037376
55.983642	2512.998546	20.042394
56.090378	2527.936103	20.047411
55.920289	2516.085707	20.052429
56.305327	2533.244421	20.057447
56.375315	2537.199162	20.062464
56.689421	2532.336691	20.067482
56.978096	2541.446620	20.072499
57.299748	2536.474641	20.077517
57.666067	2531.285062	20.082535
57.317334	2517.716686	20.087552
56.874743	2502.987548	20.092570
57.088479	2490.882025	20.097587
57.004791	2493.884278	20.102605
57.364488	2503.990831	20.107623
57.273422	2495.206672	20.112640
57.347192	2501.245846	20.117658
57.186593	2494.472230	20.122675
57.140926	2498.234476	20.127693
57.406229	2488.694045	20.132711
57.181979	2496.229790	20.137728
57.349484	2504.574351	20.142746
57.419707	2511.363859	20.147763
57.334263	2531.698105	20.152781
57.373096	2523.372150	20.157799
57.585787	2534.061633	20.162816
57.581217	2528.663683	20.167834
57.673593	2530.113738	20.172851
57.629713	2540.419281	20.177869
57.598680	2533.492947	20.182887
57.507946	2532.816542	20.187904
57.852557	2551.748158	20.192922
58.271386	2554.874450	20.197939
57.787564	2565.612723	20.202957
57.805647	2561.934114	20.207975
57.746653	2558.618216	20.212992
57.972343	2558.225321	20.218010
58.237253	2584.368415	20.223027
58.372922	2592.308866	20.228045
58.365862	2590.364985	20.233063
58.157372	2599.854919	20.238080
58.200804	2594.129942	20.243098
58.477366	2587.946985	20.248115
58.476773	2595.819412	20.253133
58.578404	2589.627176	20.258151
59.158359	2598.213056	20.263168
59.050179	2620.779356	20.268186
59.249909	2615.546812	20.273203
58.985830	2594.914502	20.278221
59.368722	2594.283045	20.283239
59.124985	2582.061923	20.288256
59.182018	2576.462058	20.293274
59.322370	2570.290988	20.298291
59.381830	2574.092372	20.303309
59.545330	2573.995953	20.308327
59.301265	2565.778925	20.313344
59.016390	2584.150482	20.318362
59.469798	2596.288504	20.323379
59.499554	2600.600474	20.328397
59.782492	2598.953328	20.333415
59.845259	2603.483647	20.338432
59.665387	2596.882252	20.343450
59.691084	2602.879218	20.348467
59.355019	2604.716594	20.353485
59.572563	2593.863615	20.358503
59.835568	2603.759261	20.363520
59.738249	2622.468544	20.368538
60.008470	2629.244736	20.373555
59.727566	2636.813925	20.378573
60.320344	2640.489795	20.383591
60.405427	2634.174694	20.388608
60.381787	2632.790397	20.393626
60.446872	2633.968418	20.398643
60.104134	2639.695991	20.403661
60.609026	2637.465942	20.408679
60.148121	2633.725535	20.413696
59.959941	2648.801505	20.418714
60.553912	2642.217871	20.423731
60.545309	2658.400117	20.428749
61.198113	2649.118364	20.433767
61.146479	2644.377513	20.438784
61.402109	2643.282475	20.443802
61.387127	2638.349165	20.448819
61.328676	2647.286616	20.453837
61.480626	2639.175354	20.458855
61.006947	2640.433353	20.463872
61.220995	2650.349717	20.468890
61.170052	2636.268868	20.473907
61.061871	2643.366046	20.478925
61.187931	2646.253357	20.483943
61.497718	2654.168216	20.488960
61.482745	2649.699239	20.493978
61.523442	2653.700383	20.498995
61.370695	2672.502344	20.504013
61.886863	2675.520653	20.509031
61.743163	2672.640550	20.514048
61.975549	2682.523197	20.519066
62.177962	2667.807580	20.524083
62.024947	2673.298710	20.529101
62.057443	2683.825765	20.534119
62.288577	2680.297144	20.539136
62.058594	2673.384926	20.544154
62.093388	2666.394902	20.549171
62.075696	2674.179453	20.554189
62.090392	2659.206105	20.559207
62.019982	2673.026306	20.564224
62.159484	2695.099455	20.569242
62.672905	2702.283098	20.574259
62.344873	2701.669717	20.579277
62.493867	2708.564593	20.584295
62.459280	2703.831143	20.589312
62.090888	2710.305648	20.594330
62.540567	2708.169944	20.599347
62.498087	2733.258059	20.604365
62.593874	2738.316390	20.609383
62.564243	2737.716290	20.614400
62.690527	2746.645906	20.619418
62.624528	2764.626609	20.624435
63.016460	2767.058222	20.629453
63.277378	2768.800901	20.634471
63.487096	2769.493446	20.639488
63.352269	2762.417834	20.644506
63.999375	2757.160128	20.649523
63.744362	2769.667307	20.654541
63.377908	2757.570846	20.659559
63.576389	2756.470087	20.664576
63.782596	2770.937140	20.669594
63.949564	2761.923192	20.674611
63.554613	2759.830804	20.679629
63.714974	2751.578536	20.684647
63.559165	2760.025480	20.689664
63.755796	2781.503915	20.694682
64.306231	2788.752344	20.699699
64.180167	2798.062843	20.704717
64.421662	2794.149634	20.709735
64.730333	2785.263822	20.714752
64.686302	2795.157970	20.719770
64.862298	2789.532464	20.724787
64.515722	2778.094471	20.729805
64.480708	2786.765941	20.734823
64.958212	2786.021408	20.739840
64.564470	2791.183879	20.744858
64.963138	2778.949546	20.749875
64.956110	2788.121085	20.754893
64.563281	2793.654642	20.759911
64.562983	2775.083489	20.764928
64.436644	2791.508545	20.769946
64.681975	2784.655122	20.774963
64.895341	2793.378852	20.779981
64.814471	2809.649178	20.784999
65.087913	2811.557498	20.790016
64.805556	2807.281668	20.795034
65.053021	2806.285403	20.800051
65.275924	2838.041236	20.805069
65.497451	2839.664456	20.810087
65.487290	2841.301161	20.815104
65.439351	2849.938583	20.820122
65.412370	2837.826903	20.825139
65.273032	2840.772280	20.830157
65.424887	2854.660632	20.835175
65.654643	2865.187495	20.840192
65.692479	2870.973515	20.845210
65.900804	2873.941364	20.850227
65.964433	2865.049939	20.855245
65.990194	2869.833287	20.860263
66.317394	2876.417113	20.865280
66.017390	2874.634198	20.870298
66.210567	2888.911399	20.875315
66.460863	2901.491077	20.880333
66.484905	2901.065950	20.885351
66.919897	2887.549221	20.890368
66.441476	2899.637543	20.895386
66.880744	2887.456649	20.900403
66.970382	2893.224275	20.905421
67.120081	2895.549490	20.910439
67.580654	2884.743741	20.915456
67.051175	2893.646580	20.920474
67.282310	2885.502223	20.925491
67.236280	2887.099587	20.930509
67.340937	2887.335904	20.935527
67.386518	2891.435707	20.940544
67.175783	2896.975428	20.945562
67.178394	2891.221459	20.950579
67.305442	2892.140258	20.955597
67.092937	2887.124162	20.960615
67.401383	2884.965911	20.965632
67.030263	2893.802425	20.970650
67.703688	2910.890283	20.975667
67.706739	2914.039297	20.980685
67.623937	2921.273148	20.985703
67.882766	2926.988813	20.990720
67.822613	2926.221712	20.995738
67.771714	2918.130244	21.000755
68.092122	2923.686921	21.005773
67.548473	2921.203357	21.010791
68.013521	2931.370534	21.015808
67.845557	2957.749367	21.020826
68.028046	2942.609441	21.025843
68.238680	2943.997870	21.030861
68.103016	2953.654126	21.035879
68.659985	2947.675464	21.040896
68.659904	2959.397005	21.045914
68.722307	2966.558852	21.050931
68.594849	2969.681416	21.055949
68.943721	2966.722024	21.060967
69.181109	2971.914110	21.065984
69.201576	2968.133441	21.071002
69.341661	2965.569164	21.076019
69.404695	2970.818014	21.081037
69.276572	2966.176511	21.086055
69.529185	2960.580012	21.091072
69.520544	2962.944788	21.096090
69.530185	2958.341149	21.101107
69.889068	2952.338923	21.106125
69.349105	2961.008111	21.111143
70.058243	2958.448612	21.116160
69.705185	2953.626185	21.121178
69.910954	2953.615491	21.126195
69.907983	2956.957625	21.131213
69.459800	2957.506943	21.136231
70.058546	2955.382989	21.141248
69.833865	2961.313600	21.146266
69.979963	2948.203989	21.151283
69.766214	2953.521405	21.156301
70.077762	2961.023949	21.161319
70.311259	2971.793561	21.166336
70.289347	2986.290245	21.171354
70.384071	2984.672785	21.176371
70.383026	2993.390723	21.181389
70.357775	2986.949230	21.186407
70.682669	2983.483981	21.191424
70.590024	3003.715316	21.196442
70.420406	2988.417007	21.201459
70.564971	3007.137567	21.206477
70.464698	3020.106361	21.211495
71.128966	3013.449344	21.216512
71.125474	3024.597903	21.221530
70.898372	3022.393100	21.226547
71.355467	3016.393516	21.231565
71.171796	3024.461761	21.236583
71.067280	3015.627956	21.241600
71.211820	3039.331789	21.246618
71.234815	3052.136152	21.251635
71.609742	3046.709952	21.256653
71.340990	3050.990475	21.261671
71.961027	3044.208477	21.266688
71.851093	3046.454183	21.271706
71.743996	3043.604377	21.276723
71.929355	3046.452438	21.281741
71.954930	3040.673754	21.286759
72.282615	3041.117695	21.291776
71.879528	3037.925875	21.296794
72.328163	3052.086213	21.301811
72.527292	3061.662409	21.306829
72.430354	3067.982169	21.311847
72.431116	3067.422308	21.316864
72.352915	3081.078419	21.321882
72.471933	3067.854290	21.326899
72.751354	3057.374408	21.331917
72.410351	3071.438884	21.336935
72.345074	3066.152348	21.341952
72.300192	3065.530741	21.346970
72.292331	3077.397352	21.351987
72.534777	3095.028268	21.357005
72.680703	3100.047331	21.362023
72.830881	3094.476372	21.367040
72.743741	3106.045883	21.372058
73.056847	3122.839597	21.377075
73.304717	3127.150512	21.382093
72.908668	3141.521774	21.387111
73.146759	3133.534793	21.392128
73.365449	3129.583145	21.397146
73.401387	3141.598072	21.402163
73.857639	3142.629015	21.407181
73.980346	3155.715793	21.412199
74.274147	3147.534567	21.417216
74.057047	3158.398061	21.422234
74.019003	3156.347816	21.427251
74.406263	3158.401933	21.432269
74.209643	3167.422749	21.437287
74.297548	3148.388558	21.442304
74.613464	3154.071647	21.447322
74.268492	3165.372009	21.452339
74.469233	3143.641720	21.457357
74.472150	3152.576407	21.462375
74.868594	3150.764981	21.467392
74.444521	3154.479096	21.472410
74.492743	3163.830302	21.477427
74.624207	3138.449795	21.482445
74.780715	3181.347186	21.487463
74.703382	3174.228421	21.492480
74.844191	3180.462878	21.497498
75.071232	3185.873274	21.502515
75.045255	3167.293296	21.507533
75.194189	3175.093278	21.512551
75.564795	3170.327175	21.517568
75.574581	3168.057221	21.522586
75.466457	3169.310951	21.527603
75.743854	3187.584992	21.532621
75.546666	3204.800117	21.537639
75.922215	3205.623542	21.542656
75.872199	3202.411924	21.547674
75.752672	3201.963664	21.552691
75.945282	3197.339954	21.557709
75.967399	3205.414837	21.562727
75.955937	3197.379302	21.567744
76.038086	3194.563940	21.572762
76.160716	3204.580017	21.577779
75.973623	3216.707052	21.582797
75.846279	3222.041776	21.587815
76.157285	3227.512719	21.592832
76.170779	3234.457583	21.597850
76.146146	3238.083663	21.602867
76.572512	3260.801137	21.607885
76.364596	3266.837358	21.612903
76.792154	3257.765494	21.617920
77.111400	3259.047030	21.622938
77.096573	3268.868547	21.627955
77.354149	3257.047694	21.632973
77.477235	3260.312372	21.637991
77.366348	3257.298590	21.643008
77.592494	3241.103162	21.648026
77.760400	3239.301146	21.653043
77.994002	3237.168994	21.658061
78.133842	3248.226315	21.663079
77.989145	3233.118521	21.668096
78.085813	3238.610320	21.673114
78.152843	3237.968638	21.678131
78.199436	3234.159965	21.683149
77.761542	3244.766316	21.688167
77.840412	3243.253020	21.693184
78.199797	3246.404633	21.698202
77.804376	3243.695739	21.703219
77.938051	3237.935731	21.708237
78.229539	3244.753955	21.713255
78.321455	3238.146938	21.718272
78.204848	3241.725228	21.723290
78.194472	3269.366697	21.728307
78.445462	3260.029924	21.733325
78.397361	3264.122472	21.738343
78.621583	3258.978576	21.743360
78.679942	3253.292423	21.748378
78.965438	3285.619523	21.753395
78.677468	3286.461656	21.758413
78.899301	3294.666963	21.763431
78.890453	3296.386961	21.768448
78.917916	3300.191056	21.773466
78.968315	3307.681807	21.778483
79.340636	3318.831465	21.783501
79.479961	3331.786516	21.788519
79.438350	3326.843215	21.793536
79.711296	3334.804276	21.798554
79.822747	3332.255300	21.803571
80.017524	3334.084957	21.808589
79.783231	3333.344643	21.813607
79.869707	3323.020085	21.818624
80.069757	3323.718979	21.823642
79.914376	3333.249598	21.828659
80.265800	3337.942662	21.833677
80.275732	3352.837565	21.838695
80.528853	3355.746925	21.843712
80.781031	3348.284266	21.848730
80.396009	3356.447765	21.853747
80.488877	3347.444149	21.858765
80.361995	3354.466200	21.863783
80.586089	3353.665097	21.868800
80.674505	3348.694790	21.873818
80.394957	3375.212454	21.878835
80.996892	3384.743546	21.883853
81.120002	3379.043891	21.888871
81.191328	3379.393202	21.893888
80.854266	3379.325758	21.898906
80.919980	3393.122138	21.903923
81.258628	3400.110193	21.908941
81.327738	3413.385176	21.913959
81.467927	3425.194123	21.918976
81.452201	3413.090763	21.923994
81.760935	3426.485998	21.929011
81.310100	3414.258873	21.934029
81.581031	3431.178394	21.939047
81.517579	3435.242422	21.944064
82.109102	3436.469926	21.949082
81.522176	3446.693568	21.954099
82.527168	3456.592737	21.959117
82.381166	3473.281207	21.964135
82.502614	3471.537629	21.969152
82.737790	3459.853392	21.974170
82.405122	3478.167172	21.979187
82.545574	3474.585446	21.984205
82.906789	3462.220156	21.989223
82.796733	3468.467444	21.994240
82.896494	3469.118746	21.999258
82.837543	3467.956937	22.004275
82.704742	3463.049921	22.009293
82.743815	3479.250736	22.014311
82.906243	3486.236061	22.019328
83.416346	3484.029051	22.024346
83.058589	3494.896339	22.029363
83.615809	3491.323690	22.034381
83.502736	3491.455448	22.039399
83.570997	3495.491427	22.044416
83.855952	3483.832017	22.049434
83.521989	3479.699957	22.054451
83.710446	3494.780846	22.059469
84.188470	3522.521582	22.064487
84.145326	3505.065674	22.069504
84.356578	3502.676553	22.074522
84.398350	3515.106154	22.079539
84.538076	3499.547956	22.084557
84.954900	3499.114598	22.089575
84.980822	3510.199198	22.094592
84.829860	3482.083347	22.099610
84.755800	3480.525223	22.104627
85.005301	3482.550575	22.109645
85.156148	3483.160365	22.114663
85.011852	3475.888749	22.119680
85.260044	3477.664715	22.124698
84.954761	3482.550988	22.129715
85.101365	3493.895944	22.134733
85.279429	3494.739028	22.139751
85.150319	3499.390686	22.144768
85.376978	3493.277427	22.149786
85.120268	3501.290274	22.154803
85.286463	3488.536330	22.159821
85.512731	3510.291977	22.164839
85.443020	3534.204017	22.169856
85.622826	3529.218944	22.174874
85.335438	3532.511353	22.179891
85.512830	3540.116269	22.184909
85.617891	3554.910608	22.189927
85.678076	3553.320056	22.194944
86.119776	3560.340367	22.199962
85.759979	3567.908477	22.204979
85.950002	3573.283395	22.209997
86.211151	3583.981543	22.215015
86.145011	3594.348747	22.220032
86.657781	3595.612900	22.225050
86.528519	3606.074400	22.230067
86.922708	3610.274658	22.235085
87.229811	3628.550216	22.240103
86.779171	3617.759107	22.245120
87.045015	3611.456258	22.250138
86.934639	3623.129205	22.255155
86.840767	3617.453902	22.260173
87.461202	3631.689532	22.265191
87.326819	3641.296396	22.270208
87.775760	3637.829009	22.275226
87.693971	3646.066171	22.280243
88.010715	3649.575700	22.285261
87.821220	3637.250881	22.290279
87.654830	3643.352432	22.295296
87.764615	3638.868656	22.300314
87.838405	3645.376972	22.305331
87.571968	3655.999755	22.310349
88.614144	3666.081498	22.315367
88.520243	3676.877358	22.320384
88.650893	3672.044456	22.325402
88.808829	3671.647969	22.330419
88.701884	3682.109376	22.335437
88.632015	3669.413190	22.340455
88.435855	3669.737025	22.345472
88.811006	3661.318860	22.350490
88.655627	3674.023685	22.355507
88.653583	3679.630772	22.360525
89.024005	3683.959387	22.365543
88.836817	3698.602158	22.370560
89.050929	3694.760572	22.375578
89.272755	3702.997987	22.380595
89.321329	3693.958576	22.385613
89.537840	3704.985837	22.390631
89.668547	3721.282392	22.395648
89.853443	3723.425145	22.400666
90.029160	3728.311143	22.405683
89.755733	3729.741053	22.410701
90.004448	3733.606723	22.415719
89.838813	3728.990481	22.420736
90.338588	3717.740673	22.425754
90.138528	3723.013175	22.430771
90.005405	3738.204922	22.435789
90.158032	3750.479778	22.440807
89.970661	3754.712005	22.445824
90.357298	3760.159223	22.450842
90.497475	3772.794816	22.455859
90.517994	3786.166336	22.460877
90.987601	3780.750222	22.465895
90.481341	3795.995024	22.470912
90.810453	3771.042636	22.475930
91.102854	3789.113332	22.480947
91.217612	3809.957903	22.485965
91.333556	3808.747089	22.490983
91.418645	3820.150875	22.496000
91.531852	3814.155846	22.501018
91.559826	3818.144630	22.506035
91.739342	3805.314603	22.511053
92.032516	3811.688704	22.516071
91.852304	3811.610692	22.521088
91.713069	3820.427520	22.526106
91.705868	3832.411528	22.531123
92.015906	3845.455728	22.536141
92.059423	3838.018654	22.541159
92.072161	3850.578913	22.546176
92.454601	3861.912726	22.551194
92.620509	3876.720151	22.556211
92.397237	3864.520026	22.561229
92.634648	3863.187167	22.566247
92.498905	3876.762541	22.571264
92.693472	3878.932458	22.576282
92.968055	3896.410549	22.581299
92.990999	3903.076195	22.586317
93.233287	3896.908228	22.591335
93.509571	3909.576560	22.596352
93.382165	3897.279464	22.601370
93.649924	3901.169984	22.606387
93.324875	3893.233546	22.611405
93.815947	3901.725396	22.616423
93.867201	3906.972179	22.621440
93.909972	3922.518902	22.626458
94.109584	3921.672997	22.631475
94.079957	3916.911388	22.636493
94.249651	3925.187457	22.641511
94.122262	3917.010862	22.646528
94.342478	3917.329676	22.651546
94.240584	3926.513233	22.656563
94.431358	3912.580064	22.661581
94.554827	3920.229904	22.666599
94.228717	3944.203841	22.671616
94.578828	3948.541005	22.676634
94.857342	3946.667088	22.681651
94.891932	3954.192654	22.686669
95.261856	3944.144865	22.691687
95.031799	3947.641275	22.696704
95.158560	3949.187753	22.701722
94.913692	3952.794881	22.706739
95.401444	3971.747694	22.711757
95.387863	3972.501212	22.716775
95.447644	3969.934293	22.721792
95.557467	3980.075036	22.726810
95.893518	3973.656108	22.731827
95.663518	3982.649447	22.736845
96.009502	4004.569472	22.741863
95.732322	4020.123493	22.746880
95.783882	4011.827118	22.751898
96.270012	4008.198384	22.756915
95.816562	4019.651937	22.761933
96.376534	4023.777276	22.766951
96.629944	4043.355919	22.771968
96.742588	4044.597647	22.776986
96.696870	4031.514491	22.782003
96.493887	4041.204199	22.787021
97.058006	4041.602410	22.792039
97.050346	4063.853797	22.797056
97.035181	4047.545829	22.802074
97.372600	4066.974003	22.807091
97.115284	4073.485637	22.812109
97.329080	4062.959624	22.817127
97.396809	4069.724636	22.822144
97.732908	4089.878663	22.827162
97.759209	4084.282152	22.832179
97.628928	4102.495896	22.837197
97.781301	4099.853417	22.842215
97.761453	4104.679723	22.847232
98.031563	4099.914591	22.852250
97.980124	4109.854896	22.857267
98.153039	4134.791569	22.862285
98.683000	4121.869907	22.867303
98.445081	4132.966266	22.872320
98.314380	4134.110021	22.877338
98.427547	4127.543211	22.882355
98.169652	4146.891901	22.887373
98.781185	4141.659304	22.892391
98.697573	4167.325838	22.897408
99.197482	4158.147008	22.902426
99.420205	4158.824084	22.907443
99.649668	4181.352605	22.912461
99.683801	4179.682434	22.917479
99.885202	4182.996573	22.922496
100.262554	4177.821165	22.927514
100.490322	4171.653915	22.932531
100.367714	4150.643781	22.937549
100.453633	4140.538070	22.942567
100.259821	4137.443723	22.947584
100.165619	4137.200704	22.952602
100.412544	4141.728601	22.957619
99.851949	4150.722727	22.962637
100.122763	4158.934573	22.967655
100.347892	4170.485164	22.972672
100.493313	4163.704342	22.977690
100.619566	4165.706449	22.982707
100.487529	4183.068587	22.987725
100.646574	4192.017050	22.992743
100.718585	4206.333992	22.997760
100.861972	4209.175425	23.002778
101.116182	4208.570098	23.007795
101.390285	4220.415398	23.012813
101.490012	4229.908740	23.017831
101.365968	4236.914183	23.022848
101.681094	4239.725274	23.027866
101.321692	4229.736007	23.032883
101.469543	4240.489553	23.037901
102.145243	4230.735552	23.042919
101.956086	4231.431085	23.047936
102.222162	4239.648087	23.052954
102.788313	4252.629835	23.057971
102.490414	4248.832957	23.062989
102.660574	4247.961193	23.068007
102.695240	4245.005059	23.073024
102.690235	4247.440692	23.078042
103.015154	4245.945698	23.083059
103.023338	4254.878967	23.088077
103.015393	4241.827976	23.093095
103.201838	4247.549400	23.098112
102.974173	4242.462137	23.103130
103.230771	4247.334541	23.108147
102.945758	4249.535333	23.113165
103.379501	4265.012279	23.118183
103.640494	4266.258253	23.123200
103.485476	4278.397743	23.128218
103.811837	4275.357180	23.133235
103.548546	4272.403032	23.138253
103.697909	4285.017445	23.143271
103.416641	4300.047598	23.148288
103.372708	4313.608181	23.153306
103.816371	4318.044169	23.158323
103.887613	4345.493741	23.163341
104.282841	4343.078030	23.168359
104.184196	4346.851250	23.173376
104.483476	4356.450675	23.178394
104.692655	4358.357606	23.183411
104.601943	4359.683359	23.188429
104.718155	4364.143154	23.193447
105.082694	4373.132964	23.198464
105.048199	4379.730350	23.203482
105.324016	4390.585300	23.208499
105.107847	4392.959782	23.213517
105.221733	4391.691781	23.218535
105.498026	4409.322142	23.223552
105.745699	4418.471847	23.228570
105.793552	4427.600637	23.233587
105.706968	4424.584581	23.238605
105.877301	4424.572265	23.243623
106.048880	4436.870517	23.248640
105.939269	4445.932027	23.253658
106.000649	4461.047059	23.258675
106.259753	4466.278583	23.263693
106.595297	4448.057039	23.268711
106.465450	4480.121780	23.273728
106.401322	4486.311884	23.278746
106.966705	4474.157344	23.283763
107.079701	4476.952271	23.288781
106.910364	4480.471837	23.293799
107.098493	4490.029474	23.298816
107.802873	4500.345549	23.303834
107.954409	4501.058816	23.308851
107.863828	4512.872077	23.313869
107.823179	4499.599492	23.318887
108.047640	4500.054632	23.323904
108.103115	4501.625152	23.328922
108.217199	4494.635181	23.333939
108.503313	4511.751019	23.338957
108.227045	4496.381440	23.343975
108.409106	4499.819714	23.348992
108.259602	4499.768907	23.354010
108.385551	4493.787261	23.359027
108.367748	4509.550889	23.364045
108.623289	4525.770176	23.369063
108.988610	4524.654326	23.374080
109.002887	4524.196515	23.379098
108.856107	4530.067600	23.384115
109.110783	4539.143381	23.389133
108.934918	4530.377199	23.394151
109.163554	4553.223341	23.399168
108.980692	4562.715154	23.404186
109.158763	4562.469264	23.409203
109.300954	4568.730038	23.414221
109.403967	4586.492782	23.419239
109.908826	4585.334185	23.424256
109.538310	4589.765019	23.429274
109.661061	4594.850605	23.434291
109.665672	4610.951988	23.439309
110.016620	4615.664815	23.444327
110.621894	4623.810221	23.449344
110.408132	4622.368772	23.454362
110.806955	4627.610336	23.459379
110.873862	4647.276073	23.464397
111.215587	4640.441739	23.469415
111.491056	4643.702791	23.474432
111.302526	4633.860628	23.479450
111.473259	4633.412002	23.484467
111.254339	4643.770502	23.489485
111.642511	4626.866113	23.494503
111.641083	4629.306727	23.499520
111.626884	4639.450282	23.504538
111.616424	4638.344943	23.509555
111.563862	4652.852970	23.514573
111.780635	4653.956274	23.519591
112.380785	4668.758057	23.524608
112.231875	4677.532870	23.529626
112.427689	4673.861009	23.534643
112.046967	4693.746452	23.539661
112.441435	4700.008506	23.544679
112.652317	4692.809527	23.549696
112.432420	4703.849371	23.554714
112.493441	4714.407344	23.559731
112.908602	4724.735533	23.564749
112.824860	4730.489183	23.569767
113.116092	4732.843655	23.574784
113.167607	4749.031530	23.579802
113.485374	4752.660048	23.584819
113.498826	4756.483745	23.589837
113.806975	4760.807993	23.594855
114.058310	4758.525454	23.599872
113.701619	4766.562161	23.604890
114.277351	4782.795740	23.609907
114.188220	4794.479438	23.614925
114.108066	4791.127974	23.619943
115.043312	4784.319919	23.624960
114.519964	4790.408456	23.629978
114.313664	4783.555556	23.634995
114.524138	4785.912356	23.640013
114.855070	4804.217252	23.645031
115.049511	4808.532350	23.650048
115.172628	4802.541604	23.655066
115.596641	4807.125086	23.660083
115.244174	4814.181525	23.665101
115.379993	4806.173188	23.670119
115.846072	4804.613082	23.675136
115.452278	4827.222692	23.680154
115.555332	4831.049712	23.685171
115.707358	4842.518781	23.690189
115.769581	4840.728930	23.695207
116.061611	4835.818605	23.700224
115.978702	4854.348256	23.705242
116.262071	4857.934448	23.710259
116.549546	4866.309281	23.715277
116.147869	4868.794022	23.720295
116.288924	4861.469486	23.725312
116.323779	4883.437832	23.730330
116.542982	4888.207948	23.735347
116.707175	4891.611858	23.740365
116.869308	4896.383532	23.745383
117.165476	4915.997944	23.750400
117.017938	4923.167037	23.755418
117.524305	4935.552892	23.760435
117.130235	4930.816153	23.765453
117.595177	4938.802224	23.770471
118.054204	4946.660133	23.775488
117.902962	4958.802677	23.780506
117.861117	4960.738958	23.785523
118.151584	4961.394247	23.790541
118.096260	4972.425985	23.795559
118.407551	4969.449596	23.800576
118.563160	4988.575868	23.805594
118.701350	4992.773530	23.810611
118.685819	4983.397481	23.815629
118.780682	4982.248334	23.820647
118.950553	5003.696861	23.825664
118.775970	5023.921524	23.830682
118.756105	5017.762575	23.835699
119.101537	5022.246892	23.840717
119.052294	5040.018775	23.845735
119.655545	5029.262785	23.850752
119.635290	5041.561322	23.855770
119.670896	5046.120860	23.860787
120.217169	5055.490519	23.865805
120.226854	5079.380389	23.870823
120.439768	5072.627789	23.875840
120.110835	5076.876676	23.880858
120.370413	5062.437764	23.885875
120.995940	5076.328186	23.890893
120.668011	5092.136560	23.895911
121.020333	5095.441706	23.900928
120.828505	5091.536139	23.905946
120.865411	5091.094652	23.910963
120.848578	5102.676469	23.915981
121.385826	5113.441476	23.920999
121.630841	5118.836193	23.926016
121.488297	5132.153915	23.931034
121.594647	5132.268719	23.936051
122.064409	5123.240780	23.941069
121.793519	5133.988146	23.946087
121.906426	5139.962623	23.951104
122.252548	5146.443891	23.956122
122.018772	5159.349508	23.961139
122.427422	5147.031356	23.966157
122.145617	5162.031319	23.971175
122.581508	5176.564246	23.976192
122.685198	5198.580327	23.981210
122.715786	5192.396042	23.986227
122.994834	5186.593577	23.991245
123.016307	5213.365828	23.996263
123.487635	5213.616404	24.001280
123.206271	5216.299054	24.006298
123.311381	5225.792507	24.011315
123.416198	5222.649777	24.016333
123.602290	5233.566997	24.021351
124.112120	5254.458464	24.026368
124.032661	5259.299308	24.031386
123.920800	5255.478527	24.036403
124.574472	5266.472064	24.041421
124.096880	5263.177509	24.046439
124.552210	5249.701451	24.051456
124.697343	5267.000092	24.056474
124.546311	5288.068530	24.061491
124.796282	5279.899342	24.066509
124.222843	5275.844168	24.071527
124.696840	5281.309383	24.076544
124.586882	5309.704855	24.081562
124.517761	5315.792952	24.086579
125.210302	5326.770659	24.091597
125.300851	5337.747838	24.096615
125.363475	5339.184176	24.101632
125.472300	5357.729594	24.106650
125.661910	5370.021273	24.111667
125.699332	5383.637458	24.116685
125.918672	5377.847151	24.121703
126.430656	5381.924878	24.126720
126.554570	5393.723441	24.131738
126.649098	5399.471504	24.136755
126.727323	5389.555254	24.141773
126.124428	5407.146178	24.146791
127.081798	5413.666331	24.151808
127.393689	5424.323895	24.156826
127.672142	5422.626607	24.161843
127.525616	5423.461619	24.166861
127.502889	5424.508088	24.171879
127.715267	5417.942062	24.176896
127.902074	5447.089225	24.181914
128.018705	5433.388632	24.186931
128.161730	5449.419182	24.191949
128.180329	5459.805515	24.196967
128.098896	5450.243992	24.201984
128.687351	5452.222653	24.207002
128.626789	5464.166332	24.212019
128.736803	5474.213124	24.217037
128.612909	5485.429408	24.222055
128.959177	5478.467569	24.227072
128.843255	5477.286280	24.232090
128.884833	5492.743021	24.237107
129.213100	5503.483376	24.242125
128.883046	5506.691501	24.247143
129.046441	5521.217410	24.252160
129.216828	5539.666247	24.257178
129.293272	5537.556213	24.262195
129.617938	5561.731030	24.267213
129.769129	5581.346216	24.272231
129.582258	5576.776639	24.277248
129.629688	5610.968985	24.282266
129.925185	5614.563587	24.287283
130.213328	5615.262602	24.292301
130.567819	5636.532260	24.297319
130.984676	5644.039968	24.302336
131.040183	5644.136403	24.307354
131.083446	5651.777510	24.312371
131.489113	5665.711483	24.317389
131.298881	5670.219140	24.322407
131.856485	5664.394095	24.327424
131.689863	5674.930876	24.332442
131.422042	5676.058418	24.337459
131.986862	5682.594334	24.342477
131.530814	5697.201501	24.347495
132.472462	5698.551290	24.352512
132.116707	5700.803344	24.357530
132.316671	5705.875747	24.362547
132.852198	5727.602684	24.367565
132.776654	5738.630821	24.372583
133.122989	5739.558052	24.377600
133.056484	5738.644990	24.382618
132.817388	5737.252903	24.387635
133.136856	5730.224900	24.392653
133.081332	5741.393056	24.397671
132.928713	5740.444218	24.402688
133.236109	5752.186351	24.407706
133.448272	5761.752215	24.412723
133.891096	5778.751412	24.417741
133.461841	5782.112222	24.422759
133.915954	5780.729222	24.427776
134.178442	5790.473033	24.432794
134.237822	5812.784739	24.437811
134.815730	5801.259869	24.442829
134.680560	5807.854805	24.447847
135.109387	5803.147197	24.452864
134.685683	5806.708303	24.457882
135.082212	5810.090167	24.462899
135.113092	5825.484823	24.467917
135.312675	5835.608003	24.472935
135.407534	5834.319406	24.477952
135.462888	5834.810802	24.482970
135.679318	5858.977189	24.487987
136.184355	5859.106839	24.493005
136.196907	5865.254498	24.498023
136.022903	5867.345817	24.503040
136.107794	5859.780063	24.508058
136.086358	5881.525615	24.513075
136.751327	5889.038906	24.518093
136.682882	5905.743144	24.523111
136.856830	5898.546566	24.528128
137.149907	5901.679761	24.533146
136.897458	5929.762846	24.538163
137.379989	5929.215413	24.543181
137.368160	5929.543086	24.548199
137.115370	5937.241915	24.553216
137.585652	5942.648520	24.558234
137.482026	5957.769821	24.563251
137.676244	5957.835856	24.568269
137.488341	5979.546443	24.573287
137.718648	5990.350965	24.578304
138.021237	5999.657116	24.583322
137.963735	6017.810267	24.588339
138.616527	6023.521831	24.593357
138.729951	6030.965282	24.598375
138.714654	6046.600102	24.603392
139.110041	6062.257641	24.608410
138.702093	6060.598106	24.613427
139.500308	6065.207938	24.618445
139.518820	6088.493467	24.623463
139.660728	6083.255935	24.628480
139.910631	6080.170963	24.633498
139.741458	6091.848772	24.638515
140.403479	6081.671027	24.643533
140.121826	6095.757546	24.648551
140.041409	6106.347310	24.653568
140.464756	6102.142957	24.658586
140.728220	6104.999942	24.663603
140.922661	6112.392637	24.668621
140.964746	6131.076002	24.673639
141.028032	6141.890114	24.678656
141.162786	6141.749802	24.683674
140.975292	6140.018391	24.688691
141.332272	6141.117931	24.693709
141.668292	6167.274394	24.698727
141.485874	6174.446670	24.703744
141.711846	6171.882250	24.708762
141.852803	6175.109150	24.713779
142.358605	6195.010657	24.718797
142.366056	6207.930431	24.723815
142.460719	6209.499373	24.728832
142.430480	6201.022017	24.733850
142.285046	6201.298926	24.738867
142.463888	6216.374194	24.743885
142.672500	6220.490067	24.748903
142.913397	6228.344507	24.753920
142.839381	6227.317284	24.758938
142.913302	6254.728418	24.763955
142.863418	6253.200277	24.768973
143.201420	6270.295294	24.773991
143.335740	6284.378611	24.779008
143.617158	6293.546286	24.784026
143.760872	6309.830794	24.789043
144.057913	6317.827207	24.794061
144.275729	6324.434121	24.799079
144.269148	6342.181530	24.804096
144.683644	6347.416363	24.809114
144.541249	6346.595740	24.814131
145.087612	6363.613903	24.819149
145.126403	6375.641874	24.824167
145.401195	6382.726882	24.829184
145.679277	6374.615880	24.834202
145.619066	6391.126327	24.839219
145.691289	6386.327053	24.844237
146.010276	6406.711742	24.849255
145.846836	6411.928690	24.854272
146.106464	6416.459879	24.859290
145.603490	6416.902188	24.864307
146.173617	6433.662127	24.869325
146.288109	6436.622542	24.874343
146.550709	6453.249034	24.879360
146.809614	6468.133330	24.884378
146.770969	6473.826614	24.889395
147.215762	6475.770086	24.894413
147.368873	6504.787750	24.899431
147.218609	6509.665486	24.904448
147.799536	6506.878551	24.909466
147.756929	6512.830817	24.914483
148.081134	6523.560338	24.919501
148.053977	6531.474186	24.924519
148.028242	6541.860684	24.929536
148.332357	6538.671373	24.934554
148.470483	6546.994215	24.939571
148.459908	6561.059195	24.944589
148.458074	6570.177756	24.949607
148.943630	6577.383960	24.954624
149.752960	6588.363345	24.959642
149.344364	6605.838048	24.964659
149.270523	6591.616244	24.969677
149.484979	6597.581193	24.974695
149.600577	6617.539838	24.979712
149.874795	6622.315178	24.984730
149.550370	6629.857645	24.989747
149.982470	6642.746199	24.994765
150.145749	6664.980124	24.999783
150.470664	6670.173165	25.004800
150.693603	6673.181860	25.009818
150.355815	6687.404189	25.014835
150.828722	6685.221797	25.019853
150.865188	6704.286371	25.024871
150.622635	6718.782023	25.029888
150.955938	6718.767196	25.034906
151.157249	6734.280277	25.039923
152.006687	6746.899918	25.044941
152.507473	6739.184296	25.049959
152.533776	6751.626508	25.054976
153.063526	6742.634201	25.059994
153.126928	6731.417731	25.065011
153.061487	6723.297159	25.070029
153.134974	6705.895978	25.075047
153.137643	6710.107439	25.080064
153.602719	6699.056948	25.085082
153.419908	6706.484696	25.090099
153.504924	6698.902373	25.095117
153.488311	6699.136740	25.100135
153.387644	6702.899832	25.105152
153.427228	6718.038758	25.110170
153.043759	6730.299010	25.115187
153.513045	6747.178330	25.120205
153.854759	6765.224637	25.125223
153.872513	6768.121557	25.130240
154.265411	6770.213039	25.135258
153.923700	6796.752669	25.140275
154.017037	6806.404568	25.145293
154.432959	6822.918698	25.150311
154.436180	6842.409487	25.155328
154.699111	6850.096786	25.160346
154.713022	6870.783719	25.165363
155.290730	6880.732079	25.170381
155.287636	6887.771090	25.175399
155.799112	6902.967679	25.180416
156.114153	6901.756416	25.185434
156.328729	6910.903996	25.190451
156.460209	6928.030706	25.195469
156.677870	6930.749712	25.200487
156.545126	6935.078903	25.205504
156.686641	6944.340958	25.210522
156.899054	6941.607754	25.215539
156.679408	6952.500677	25.220557
156.962748	6962.940341	25.225575
156.902943	6965.266528	25.230592
157.637323	6987.578231	25.235610
157.625962	7005.068068	25.240627
157.200088	7005.128282	25.245645
157.662580	7016.201509	25.250663
157.458276	7027.465254	25.255680
158.204991	7040.666793	25.260698
158.351599	7055.618244	25.265715
158.424255	7065.331998	25.270733
158.875983	7064.474595	25.275751
159.145478	7087.599634	25.280768
159.548903	7072.324310	25.285786
159.630121	7083.426720	25.290803
159.667311	7075.386666	25.295821
159.824252	7075.164711	25.300839
159.977962	7100.900790	25.305856
160.275130	7101.728335	25.310874
160.267091	7100.620059	25.315891
160.111631	7093.085158	25.320909
160.311263	7105.256438	25.325927
160.460991	7122.505568	25.330944
160.949910	7124.350474	25.335962
160.853446	7137.058211	25.340979
160.676583	7140.089742	25.345997
161.247803	7144.739772	25.351015
161.222340	7165.244580	25.356032
161.332675	7161.435054	25.361050
161.410357	7173.588734	25.366067
161.569274	7191.598005	25.371085
161.954498	7187.152369	25.376103
161.980830	7201.948205	25.381120
162.063761	7217.638839	25.386138
161.790687	7225.214845	25.391155
162.188394	7237.283403	25.396173
162.796033	7251.550853	25.401191
162.678643	7257.504730	25.406208
162.715178	7262.745620	25.411226
162.896912	7278.101019	25.416243
162.983690	7285.092278	25.421261
163.347128	7301.691980	25.426279
163.305247	7316.432249	25.431296
163.614767	7316.585171	25.436314
163.654992	7340.172970	25.441331
163.889734	7352.453626	25.446349
164.259361	7357.924614	25.451367
164.185058	7375.670199	25.456384
164.252584	7377.520184	25.461402
164.322713	7395.215936	25.466419
164.728120	7417.330582	25.471437
164.953165	7420.686398	25.476455
165.266740	7441.351342	25.481472
165.431636	7453.180517	25.486490
165.690739	7454.884656	25.491507
166.081916	7451.009753	25.496525
166.490454	7477.003622	25.501543
166.300914	7478.967766	25.506560
166.374803	7480.274851	25.511578
166.494670	7477.188255	25.516595
166.449654	7479.283674	25.521613
166.890087	7503.393129	25.526631
166.801434	7513.834769	25.531648
166.940222	7524.690124	25.536666
167.427470	7546.011713	25.541683
167.083919	7551.840826	25.546701
167.427383	7558.663778	25.551719
167.441215	7582.506755	25.556736
168.041125	7578.990340	25.561754
168.082771	7609.683192	25.566771
168.194785	7615.943478	25.571789
168.482156	7614.242125	25.576807
168.477191	7635.924763	25.581824
168.744590	7633.205196	25.586842
169.168908	7644.397801	25.591859
169.354637	7671.427479	25.596877
169.287282	7664.918165	25.601895
169.201263	7687.007277	25.606912
169.934864	7686.008757	25.611930
170.031500	7695.303084	25.616947
170.199167	7703.739798	25.621965
170.336081	7696.372100	25.626983
170.228759	7713.075225	25.632000
170.419706	7724.061504	25.637018
170.566240	7736.430282	25.642035
170.585489	7753.821377	25.647053
170.998141	7758.599394	25.652071
170.829149	7778.094591	25.657088
171.080393	7791.720453	25.662106
171.405543	7803.802223	25.667123
171.752666	7816.106415	25.672141
172.342422	7822.094092	25.677159
172.192191	7827.366029	25.682176
172.442859	7827.983132	25.687194
172.416801	7850.823392	25.692212
172.889844	7854.275368	25.697229
173.081567	7847.333304	25.702247
173.062010	7863.994519	25.707264
173.354050	7872.946346	25.712282
173.464477	7877.786152	25.717300
173.510287	7892.596743	25.722317
173.653952	7893.359121	25.727335
173.815364	7903.617141	25.732352
173.915769	7912.632160	25.737370
174.329906	7915.970228	25.742388
174.146952	7925.016323	25.747405
174.710008	7940.351890	25.752423
174.433819	7958.363045	25.757440
174.412978	7947.605422	25.762458
174.902819	7959.286771	25.767476
174.888336	7984.219574	25.772493
175.049086	7987.344339	25.777511
175.299365	8007.867686	25.782528
175.489451	8016.815176	25.787546
175.437862	8028.228461	25.792564
175.359825	8054.178449	25.797581
175.824458	8040.541353	25.802599
176.489731	8073.371256	25.807616
176.608478	8072.631046	25.812634
176.969357	8084.218805	25.817652
176.845085	8103.455761	25.822669
176.960162	8119.928024	25.827687
177.204082	8118.490563	25.832704
177.283765	8139.594393	25.837722
177.199833	8147.025379	25.842740
177.394945	8163.523057	25.847757
178.280690	8181.025849	25.852775
178.164914	8194.730819	25.857792
178.198932	8186.394578	25.862810
178.520480	8201.882148	25.867828
178.568886	8210.048205	25.872845
179.054267	8218.612276	25.877863
178.888530	8241.943242	25.882880
179.172373	8241.305703	25.887898
179.499343	8254.963560	25.892916
179.468912	8270.863789	25.897933
179.774912	8267.458802	25.902951
179.737836	8285.447358	25.907968
180.334330	8307.284363	25.912986
180.138541	8299.541313	25.918004
180.424174	8308.803198	25.923021
180.532100	8336.112299	25.928039
180.559728	8340.971442	25.933056
180.965650	8357.899192	25.938074
181.407133	8366.592680	25.943092
181.461809	8370.049314	25.948109
181.696832	8376.038321	25.953127
181.826689	8398.051009	25.958144
181.814950	8403.823243	25.963162
182.005552	8425.566801	25.968180
182.187693	8435.074274	25.973197
182.407575	8447.726065	25.978215
182.845516	8455.568752	25.983232
183.062868	8450.668472	25.988250
183.330843	8457.805954	25.993268
183.365668	8480.009314	25.998285
183.791676	8477.048372	26.003303
184.161507	8488.501838	26.008320
184.120512	8489.445197	26.013338
184.149394	8486.179681	26.018356
184.465783	8508.702023	26.023373
184.501157	8514.273541	26.028391
184.693008	8526.309366	26.033408
184.814794	8536.774405	26.038426
185.417997	8535.546916	26.043444
185.306755	8548.280280	26.048461
185.397698	8552.968347	26.053479
185.600702	8566.622540	26.058496
186.251367	8573.766154	26.063514
186.666575	8559.728782	26.068532
186.418703	8568.800934	26.073549
186.744289	8566.222823	26.078567
186.719111	8557.565358	26.083584
186.906143	8559.349265	26.088602
186.986746	8568.852330	26.093620
186.991237	8585.626902	26.098637
187.381549	8590.318287	26.103655
187.515197	8598.294815	26.108672
187.521537	8599.658050	26.113690
187.381363	8613.773050	26.118708
187.498096	8635.567696	26.123725
187.826005	8630.271811	26.128743
187.871860	8652.842209	26.133760
187.802142	8674.799254	26.138778
188.214551	8681.606577	26.143796
188.091332	8691.896386	26.148813
188.701644	8710.399122	26.153831
188.713678	8730.268854	26.158848
188.904465	8744.882215	26.163866
189.311350	8766.925257	26.168884
189.216400	8782.742928	26.173901
189.608820	8786.643219	26.178919
190.224292	8821.598544	26.183936
190.407668	8832.439553	26.188954
190.274292	8823.321714	26.193972
190.369545	8859.630417	26.198989
190.468329	8864.412587	26.204007
190.908090	8884.054305	26.209024
190.917407	8893.994679	26.214042
191.354240	8911.211712	26.219060
191.503445	8928.980391	26.224077
191.719246	8936.503213	26.229095
191.688434	8946.434497	26.234112
191.643108	8968.142166	26.239130
192.408301	8967.468388	26.244148
192.623133	8995.294996	26.249165
192.495563	9002.914755	26.254183
192.886709	9024.878839	26.259200
193.120500	9033.238385	26.264218
193.307600	9049.614646	26.269236
193.116669	9068.802347	26.274253
193.374159	9075.411740	26.279271
194.158674	9090.006084	26.284288
194.289637	9106.688631	26.289306
194.723545	9114.304677	26.294324
194.695033	9123.942678	26.299341
195.074522	9123.036462	26.304359
195.181123	9126.194031	26.309376
195.337537	9139.909190	26.314394
195.896772	9142.949439	26.319412
195.650160	9143.707050	26.324429
196.040656	9166.986850	26.329447
196.226483	9182.584450	26.334464
196.470570	9183.490985	26.339482
196.609327	9184.696911	26.344500
196.598065	9195.811358	26.349517
196.430607	9200.016933	26.354535
196.841639	9221.872456	26.359552
196.849945	9233.984043	26.364570
197.052032	9235.481189	26.369588
197.003689	9254.256441	26.374605
197.159392	9268.093919	26.379623
197.680362	9293.049003	26.384640
197.643264	9311.386090	26.389658
198.050463	9326.444714	26.394676
198.166303	9348.806041	26.399693
198.284629	9366.285719	26.404711
198.441225	9381.643375	26.409728
198.792415	9400.802552	26.414746
199.146717	9411.416430	26.419764
199.346017	9421.450985	26.424781
199.914762	9429.894817	26.429799
200.100669	9433.566305	26.434816
200.247097	9438.636158	26.439834
200.741241	9453.972769	26.444852
200.598726	9468.105454	26.449869
200.821691	9463.515074	26.454887
200.948468	9459.254088	26.459904
200.860428	9491.886877	26.464922
201.255208	9482.676665	26.469940
201.341012	9506.817839	26.474957
201.564568	9525.116043	26.479975
201.759629	9527.850264	26.484992
201.965228	9541.912892	26.490010
202.038663	9563.883744	26.495028
202.041241	9580.844001	26.500045
202.370856	9595.513976	26.505063
202.619256	9608.893750	26.510080
202.858167	9633.619493	26.515098
202.970377	9650.314373	26.520116
202.962194	9665.382875	26.525133
203.491244	9685.784352	26.530151
203.479875	9700.413090	26.535168
203.367506	9708.293766	26.540186
203.937689	9725.274607	26.545204
203.764166	9740.575302	26.550221
204.063687	9764.771351	26.555239
204.487943	9792.638794	26.560256
204.394234	9804.648728	26.565274
205.068866	9828.586757	26.570292
205.211573	9849.198004	26.575309
205.552698	9856.493388	26.580327
206.082929	9869.373095	26.585344
205.857253	9896.647836	26.590362
206.283217	9907.887463	26.595380
206.722466	9916.559332	26.600397
206.714040	9920.024366	26.605415
207.275838	9937.118675	26.610432
207.141935	9959.902589	26.615450
207.461506	9963.788428	26.620468
207.587290	9973.328979	26.625485
207.850279	9998.616889	26.630503
207.963828	9997.805769	26.635520
208.347416	10026.490111	26.640538
208.568511	10034.964927	26.645556
208.425864	10041.625871	26.650573
208.539411	10068.272974	26.655591
209.105222	10071.475377	26.660608
208.941403	10090.102120	26.665626
209.305746	10105.808980	26.670644
209.409545	10133.498379	26.675661
209.734541	10147.526847	26.680679
210.072186	10158.194392	26.685696
210.272535	10175.438479	26.690714
210.480110	10177.426348	26.695732
210.826816	10190.807698	26.700749
211.048586	10210.237367	26.705767
211.524284	10213.026954	26.710784
211.532757	10238.295854	26.715802
211.880593	10228.420255	26.720820
212.057437	10231.159184	26.725837
212.381943	10255.515698	26.730855
213.169623	10248.852231	26.735872
212.723221	10264.153613	26.740890
212.466413	10258.613508	26.745908
213.013758	10283.747754	26.750925
213.181761	10292.860087	26.755943
213.402904	10292.812602	26.760960
213.216750	10311.592962	26.765978
213.594040	10326.532228	26.770996
213.715450	10346.860115	26.776013
213.650632	10362.976075	26.781031
214.409755	10363.673121	26.786048
214.114780	10397.439260	26.791066
214.430277	10395.386371	26.796084
214.688742	10416.691335	26.801101
214.828781	10430.183444	26.806119
215.245393	10430.247818	26.811136
215.246812	10458.543922	26.816154
215.866849	10472.523927	26.821172
216.102004	10484.294127	26.826189
216.319228	10501.843785	26.831207
216.569778	10506.571439	26.836224
216.053427	10532.064585	26.841242
216.547470	10549.861597	26.846260
216.758195	10555.229977	26.851277
217.066543	10571.517661	26.856295
217.646439	10583.593335	26.861312
217.686421	10612.365438	26.866330
218.030544	10619.627593	26.871348
218.271870	10632.268915	26.876365
218.240860	10640.259495	26.881383
219.041849	10639.972046	26.886400
218.974948	10662.594642	26.891418
219.164177	10678.187630	26.896436
219.278592	10677.033664	26.901453
219.514024	10703.556128	26.906471
219.896685	10706.550237	26.911488
220.108434	10733.679293	26.916506
220.354563	10747.508628	26.921524
220.612801	10759.754958	26.926541
220.963576	10766.526100	26.931559
221.014410	10779.974949	26.936576
220.789908	10791.235236	26.941594
221.085341	10809.703433	26.946612
221.592584	10807.683407	26.951629
221.633313	10828.620779	26.956647
222.379902	10850.438850	26.961664
222.451729	10858.262085	26.966682
222.557925	10866.690157	26.971700
223.016987	10874.462022	26.976717
222.694822	10890.817185	26.981735
223.073665	10895.776628	26.986752
223.451496	10905.940172	26.991770
223.655916	10934.443055	26.996788
223.823291	10942.608187	27.001805
223.843509	10958.386925	27.006823
224.240933	10970.156669	27.011840
224.309760	10987.155525	27.016858
224.565236	11004.234634	27.021876
225.077288	11005.479856	27.026893
224.996990	11027.803467	27.031911
225.579457	11043.530355	27.036928
225.456663	11062.394081	27.041946
225.681490	11071.795245	27.046964
226.036362	11087.541663	27.051981
226.037296	11105.398712	27.056999
226.610858	11110.038515	27.062016
227.150445	11140.933983	27.067034
226.883310	11147.333933	27.072052
227.159918	11149.003288	27.077069
226.994387	11177.860779	27.082087
227.425490	11179.802389	27.087104
227.582263	11202.120947	27.092122
227.790487	11218.803177	27.097140
228.505821	11231.187831	27.102157
228.440614	11248.046040	27.107175
228.949149	11262.621815	27.112192
228.800654	11285.142179	27.117210
228.714055	11286.678555	27.122228
229.338040	11305.451479	27.127245
229.131916	11316.148198	27.132263
229.451476	11324.105615	27.137280
229.674696	11355.586308	27.142298
229.672127	11390.246832	27.147316
229.611382	11397.150835	27.152333
230.325329	11407.976834	27.157351
230.401893	11427.626556	27.162368
231.016858	11466.780358	27.167386
231.062280	11482.368742	27.172404
231.171495	11499.003812	27.177421
231.632529	11522.343934	27.182439
232.118560	11536.228060	27.187456
232.235932	11562.535904	27.192474
232.308649	11567.899069	27.197492
233.101270	11588.058546	27.202509
232.919833	11601.574822	27.207527
233.486055	11598.374296	27.212544
234.074564	11615.369884	27.217562
234.256289	11630.545933	27.222580
234.887818	11633.770101	27.227597
234.988245	11642.331096	27.232615
235.101367	11638.681543	27.237632
235.373481	11644.627055	27.242650
235.160139	11666.887666	27.247668
235.981798	11661.111373	27.252685
235.589162	11665.105065	27.257703
236.063081	11681.393309	27.262720
236.144705	11698.168645	27.267738
236.281841	11697.730112	27.272756
236.001338	11712.867592	27.277773
236.261060	11740.463892	27.282791
236.693031	11765.552571	27.287808
236.707261	11780.349144	27.292826
237.040630	11800.134146	27.297844
236.959450	11828.577877	27.302861
237.102308	11847.568797	27.307879
237.622718	11861.913118	27.312896
237.840542	11898.714242	27.317914
238.285281	11915.481017	27.322932
238.396877	11923.407706	27.327949
238.459396	11966.099091	27.332967
238.890938	11978.435891	27.337984
239.176576	11991.839082	27.343002
239.532802	12028.729505	27.348020
240.250316	12027.352111	27.353037
239.796268	12045.030126	27.358055
240.384420	12069.305660	27.363072
240.899296	12083.272156	27.368090
241.002107	12101.158383	27.373108
241.543714	12103.842883	27.378125
241.686828	12126.443081	27.383143
242.017097	12122.522771	27.388160
242.484087	12129.062581	27.393178
242.614394	12146.800934	27.398196
243.010954	12157.874476	27.403213
243.025848	12149.953722	27.408231
243.409443	12161.673057	27.413248
243.364176	12188.065520	27.418266
243.408625	12196.353231	27.423284
243.644450	12212.757772	27.428301
243.682249	12227.926653	27.433319
244.119788	12240.778689	27.438336
244.332088	12258.981039	27.443354
244.408569	12271.263283	27.448372
244.713477	12281.987290	27.453389
244.304171	12307.055885	27.458407
244.905736	12322.688702	27.463424
244.755784	12334.305663	27.468442
244.975238	12361.148639	27.473460
245.528474	12384.551201	27.478477
245.652070	12404.158893	27.483495
245.871476	12434.748928	27.488512
246.690002	12452.798550	27.493530
246.401766	12475.795095	27.498548
246.798179	12493.492226	27.503565
246.996938	12524.393098	27.508583
247.326208	12539.566112	27.513600
247.824372	12570.104044	27.518618
247.842010	12589.798010	27.523636
248.067188	12597.277680	27.528653
248.299254	12636.312454	27.533671
248.668237	12646.082282	27.538688
248.964276	12654.290055	27.543706
249.259281	12675.880335	27.548724
249.586089	12701.975021	27.553741
249.634539	12712.825200	27.558759
250.043581	12741.255722	27.563776
250.374851	12751.810240	27.568794
250.638553	12788.581393	27.573812
250.933378	12794.164320	27.578829
251.183194	12822.438512	27.583847
251.143151	12837.401804	27.588864
251.806658	12840.971534	27.593882
251.759659	12868.549538	27.598900
252.214866	12882.925243	27.603917
252.443678	12898.958199	27.608935
252.925654	12911.897185	27.613952
253.401199	12935.378778	27.618970
253.147000	12951.973759	27.623988
253.855939	12969.586687	27.629005
253.916028	12981.804424	27.634023
254.235739	12989.445926	27.639040
254.509423	13007.271049	27.644058
254.553451	13023.386657	27.649076
254.862312	13035.495576	27.654093
255.328791	13052.285157	27.659111
255.318436	13073.040863	27.664128
255.628622	13089.530130	27.669146
255.786068	13105.924895	27.674164
256.129116	13127.392813	27.679181
256.462609	13148.967912	27.684199
256.478919	13151.514841	27.689216
256.699080	13172.522523	27.694234
256.989684	13201.922021	27.699252
257.278382	13213.930406	27.704269
257.642163	13236.401943	27.709287
257.743037	13262.990256	27.714304
257.935080	13274.869687	27.719322
258.152642	13304.128591	27.724340
258.452734	13318.836010	27.729357
258.305982	13348.419912	27.734375
258.961452	13369.798716	27.739392
259.418867	13387.567114	27.744410
259.585411	13406.149410	27.749428
260.004193	13418.583972	27.754445
260.496929	13445.273295	27.759463
260.339778	13459.473355	27.764480
260.596473	13465.691548	27.769498
260.558086	13491.715483	27.774516
261.273820	13501.795696	27.779533
261.326952	13527.273533	27.784551
261.262392	13551.596903	27.789568
262.105898	13565.927973	27.794586
262.226693	13574.152564	27.799604
262.949173	13599.891809	27.804621
262.775979	13611.251945	27.809639
263.030787	13627.519272	27.814656
263.413153	13638.299145	27.819674
263.427873	13654.913444	27.824692
263.853594	13668.667561	27.829709
263.610154	13689.694206	27.834727
263.550374	13722.901343	27.839744
263.915228	13738.181487	27.844762
264.092890	13765.155036	27.849780
264.435167	13793.407771	27.854797
264.715051	13822.942534	27.859815
264.616647	13841.857476	27.864832
265.781427	13864.441795	27.869850
266.319439	13890.421563	27.874868
266.384085	13914.424726	27.879885
266.786264	13943.580219	27.884903
267.174040	13946.336940	27.889920
267.500836	13952.225423	27.894938
267.711068	13996.444425	27.899956
268.200298	13995.906690	27.904973
268.182298	14006.048566	27.909991
268.011447	14032.853224	27.915008
268.260286	14041.890507	27.920026
268.613305	14070.168738	27.925044
269.243736	14082.601935	27.930061
269.618379	14105.744188	27.935079
269.670723	14116.293681	27.940096
270.092632	14136.486094	27.945114
270.079398	14156.334405	27.950132
270.604468	14171.125193	27.955149
270.494904	14197.522885	27.960167
271.066236	14231.487197	27.965184
271.460412	14229.830555	27.970202
271.399505	14248.615283	27.975220
271.850600	14282.399435	27.980237
272.108593	14301.051168	27.985255
271.887629	14326.808771	27.990272
272.201890	14354.260276	27.995290
272.351804	14376.184089	28.000308
272.810361	14400.103977	28.005325
272.756537	14435.941692	28.010343
272.979333	14473.750890	28.015360
273.671635	14493.229331	28.020378
273.579955	14528.616503	28.025396
274.218047	14555.341948	28.030413
274.691553	14569.235492	28.035431
274.852670	14591.914164	28.040448
275.263022	14621.335848	28.045466
275.366320	14643.630176	28.050484
275.818111	14674.141922	28.055501
276.028568	14681.948835	28.060519
276.697326	14708.215610	28.065536
276.978951	14721.893573	28.070554
276.811152	14760.508639	28.075572
277.299522	14771.534928	28.080589
277.544152	14794.636608	28.085607
277.591118	14813.497143	28.090624
278.419963	14826.057298	28.095642
278.399871	14859.649444	28.100660
278.484383	14886.777349	28.105677
278.943855	14901.833363	28.110695
279.012647	14923.076340	28.115712
279.489405	14943.402527	28.120730
279.717341	14971.523339	28.125748
280.011328	14989.314194	28.130765
280.387515	15005.525027	28.135783
280.766459	15037.362229	28.140800
280.882618	15053.111776	28.145818
280.848952	15064.153598	28.150836
280.982920	15079.430603	28.155853
281.604641	15108.168966	28.160871
281.529926	15124.394529	28.165888
282.284723	15149.688063	28.170906
282.306779	15175.473043	28.175924
282.649133	15191.850397	28.180941
282.771989	15220.293154	28.185959
283.140925	15240.793545	28.190976
283.560990	15252.814833	28.195994
283.386530	15290.174651	28.201012
283.791943	15322.800737	28.206029
283.942139	15350.542636	28.211047
284.129767	15376.027938	28.216064
284.719444	15408.300681	28.221082
285.099320	15448.164873	28.226100
285.421832	15464.432309	28.231117
285.963232	15490.650474	28.236135
285.782637	15512.548471	28.241152
287.083447	15530.480887	28.246170
287.061147	15547.774595	28.251188
287.191224	15569.115454	28.256205
288.007099	15579.200913	28.261223
287.877095	15611.641818	28.266240
288.542560	15622.051589	28.271258
288.653306	15642.818931	28.276276
289.003682	15655.367376	28.281293
289.155679	15676.236688	28.286311
289.223172	15690.672643	28.291328
289.604924	15707.269371	28.296346
289.534990	15732.057070	28.301364
289.380942	15757.485946	28.306381
289.687706	15786.608499	28.311399
290.012638	15810.402819	28.316416
290.491974	15844.440858	28.321434
290.820361	15879.611834	28.326452
291.392522	15906.043072	28.331469
291.792861	15931.695826	28.336487
292.158738	15961.492911	28.341504
292.563097	15976.106712	28.346522
292.707553	16010.324928	28.351540
292.930543	16018.978307	28.356557
293.634512	16047.580233	28.361575
293.356173	16076.065547	28.366592
294.079590	16094.209032	28.371610
294.322694	16114.233287	28.376628
294.567171	16136.329813	28.381645
295.062102	16149.475710	28.386663
294.917788	16176.438678	28.391680
295.314613	16197.367495	28.396698
295.359688	16227.088830	28.401716
295.625739	16259.623186	28.406733
295.748067	16273.708595	28.411751
295.789072	16310.715206	28.416768
296.506730	16335.524994	28.421786
296.767742	16364.835805	28.426804
297.331059	16381.541914	28.431821
297.749086	16406.609353	28.436839
298.077068	16429.002959	28.441856
298.541168	16455.019525	28.446874
298.575018	16472.043306	28.451892
298.683179	16505.523077	28.456909
299.378264	16513.446233	28.461927
299.706686	16540.448323	28.466944
299.828192	16566.006293	28.471962
300.196879	16574.645352	28.476980
300.444047	16596.513525	28.481997
301.110148	16604.282331	28.487015
301.086438	16632.494857	28.492032
301.395803	16637.588131	28.497050
302.077131	16653.754917	28.502068
302.090125	16678.583931	28.507085
302.593663	16686.868218	28.512103
302.313569	16710.962392	28.517120
302.680949	16728.777692	28.522138
303.257935	16739.018397	28.527156
303.490356	16774.292259	28.532173
304.020672	16789.286304	28.537191
303.876773	16814.972043	28.542208
304.841588	16831.427877	28.547226
304.761295	16847.307750	28.552244
304.777684	16859.166808	28.557261
305.560606	16875.551868	28.562279
305.542527	16915.677666	28.567296
305.627644	16923.227391	28.572314
305.915314	16945.872660	28.577332
305.915335	16990.197540	28.582349
306.474534	17006.482572	28.587367
306.902714	17036.328059	28.592384
307.220038	17057.808565	28.597402
307.367534	17085.205526	28.602420
307.805352	17121.855248	28.607437
308.258135	17143.338704	28.612455
308.124313	17184.098966	28.617472
308.426616	17200.710336	28.622490
308.727524	17232.214803	28.627508
309.259055	17271.427924	28.632525
309.740941	17288.592884	28.637543
309.779700	17324.379067	28.642560
310.250107	17353.508891	28.647578
310.644562	17380.162583	28.652596
310.506223	17411.312826	28.657613
310.945922	17429.312381	28.662631
311.060684	17470.535072	28.667648
311.526426	17497.793453	28.672666
312.081689	17527.738625	28.677684
311.806343	17558.352244	28.682701
312.536812	17589.416027	28.687719
312.889560	17630.235706	28.692736
313.445534	17659.589937	28.697754
313.498985	17689.728641	28.702772
313.508635	17719.627176	28.707789
314.228493	17747.293198	28.712807
314.680663	17784.109098	28.717824
315.060508	17800.812293	28.722842
315.181839	17841.350761	28.727860
315.720734	17879.183373	28.732877
316.513160	17882.209651	28.737895
315.952279	17925.674539	28.742912
316.523606	17956.700684	28.747930
316.837901	17982.481194	28.752948
317.115323	18006.147842	28.757965
317.366567	18037.373607	28.762983
317.670114	18051.168950	28.768000
318.414120	18081.410221	28.773018
318.644977	18113.659308	28.778036
318.781726	18138.988650	28.783053
319.474010	18162.147218	28.788071
319.523027	18191.661811	28.793088
319.935340	18216.372001	28.798106
319.997492	18245.789947	28.803124
320.189659	18284.271856	28.808141
320.672553	18306.349249	28.813159
320.959483	18329.518276	28.818176
321.198877	18362.095870	28.823194
321.482201	18381.785233	28.828212
321.853497	18406.833495	28.833229
322.496235	18427.450261	28.838247
322.911094	18452.149350	28.843264
323.350597	18470.019247	28.848282
323.533692	18493.979597	28.853300
323.569894	18520.070125	28.858317
324.267100	18534.045154	28.863335
324.634637	18565.277925	28.868352
324.699598	18583.895496	28.873370
325.033243	18606.738790	28.878388
325.272297	18628.180682	28.883405
325.561895	18649.396727	28.888423
325.953603	18685.701307	28.893440
326.091880	18703.294935	28.898458
326.298972	18730.836103	28.903476
326.648376	18773.895893	28.908493
326.788971	18811.139136	28.913511
326.849011	18844.083058	28.918528
327.190384	18878.706601	28.923546
327.944879	18909.415816	28.928564
327.781471	18953.610603	28.933581
328.393851	18983.042991	28.938599
328.964077	19033.057851	28.943616
329.298714	19056.008790	28.948634
329.777629	19091.825385	28.953652
329.712749	19129.541503	28.958669
330.214699	19149.468363	28.963687
330.686680	19194.197224	28.968704
330.819177	19229.180729	28.973722
331.214966	19254.850451	28.978740
331.348981	19296.799619	28.983757
332.074463	19326.929585	28.988775
332.304656	19355.104811	28.993792
332.309152	19386.747478	28.998810
332.791567	19423.664494	29.003828
333.377144	19456.196504	29.008845
333.727901	19490.681056	29.013863
334.148140	19520.691559	29.018880
334.505995	19553.849361	29.023898
334.928596	19589.069438	29.028916
334.995551	19619.690209	29.033933
335.602432	19644.556398	29.038951
335.715960	19683.046663	29.043968
336.225805	19707.973117	29.048986
336.903640	19730.773708	29.054004
336.883383	19764.298636	29.059021
337.384551	19784.964132	29.064039
338.181505	19821.065526	29.069056
338.464234	19836.431140	29.074074
338.720265	19855.825676	29.079092
339.273516	19866.598770	29.084109
339.446766	19881.222697	29.089127
339.922374	19920.339419	29.094144
339.703312	19949.797386	29.099162
340.681631	19952.987245	29.104180
340.388918	20001.219662	29.109197
340.792041	20013.578285	29.114215
341.215398	20052.790652	29.119232
341.451640	20075.016772	29.124250
341.863173	20101.315763	29.129268
341.754197	20120.211286	29.134285
342.292161	20165.664891	29.139303
342.705668	20187.858723	29.144320
342.601296	20215.114880	29.149338
342.971666	20246.113885	29.154356
343.281567	20282.307782	29.159373
343.544718	20310.575343	29.164391
343.616143	20349.446139	29.169408
344.105080	20381.327523	29.174426
344.562086	20407.274246	29.179444
344.503308	20468.009883	29.184461
345.299481	20491.291701	29.189479
345.671743	20526.624548	29.194496
345.660435	20570.393348	29.199514
346.302535	20596.435903	29.204532
346.194247	20637.610300	29.209549
346.996567	20673.477768	29.214567
347.544003	20704.607595	29.219584
347.962153	20748.863980	29.224602
348.405831	20771.536004	29.229620
349.018888	20809.648391	29.234637
349.479237	20816.811572	29.239655
350.044203	20850.629811	29.244672
350.232220	20886.034846	29.249690
350.884950	20896.637682	29.254708
351.016289	20921.103518	29.259725
351.429060	20933.901070	29.264743
351.603239	20964.872339	29.269760
352.177486	20997.741876	29.274778
352.476708	21011.639717	29.279796
352.648548	21042.641470	29.284813
352.990487	21058.441425	29.289831
353.756779	21087.278272	29.294848
354.246159	21103.998233	29.299866
354.537700	21106.054775	29.304884
354.688451	21138.817986	29.309901
355.541185	21160.354094	29.314919
355.687627	21177.599005	29.319936
356.000078	21195.748224	29.324954
356.471983	21218.184446	29.329972
356.530297	21244.978711	29.334989
357.006225	21257.487035	29.340007
357.377299	21283.638501	29.345024
357.490320	21303.912819	29.350042
357.752436	21330.749225	29.355060
357.737972	21356.296053	29.360077
358.015870	21384.465252	29.365095
358.648899	21417.615985	29.370112
358.745598	21466.138279	29.375130
359.268526	21482.856231	29.380148
359.810119	21516.192531	29.385165
359.802949	21551.296994	29.390183
360.294273	21574.205024	29.395200
360.157264	21611.114131	29.400218
360.639287	21645.559381	29.405236
360.719788	21688.589147	29.410253
361.380597	21725.201163	29.415271
361.610975	21771.537645	29.420288
361.715784	21804.579338	29.425306
362.394386	21844.275587	29.430324
362.365801	21894.732193	29.435341
362.685147	21930.894989	29.440359
363.626063	21976.105643	29.445376
363.839235	22024.391164	29.450394
364.357239	22056.423870	29.455412
364.384311	22091.894303	29.460429
364.966355	22129.956489	29.465447
365.471943	22170.421515	29.470464
365.561271	22217.816776	29.475482
366.168811	22241.701357	29.480500
366.350342	22283.929230	29.485517
366.696976	22317.264645	29.490535
367.649279	22356.923197	29.495552
367.594040	22392.639623	29.500570
367.869612	22415.893465	29.505588
368.069559	22461.377616	29.510605
368.449509	22497.448059	29.515623
368.758813	22537.340969	29.520640
369.075133	22578.268664	29.525658
369.599245	22606.347208	29.530676
370.100825	22650.031970	29.535693
370.357503	22690.894113	29.540711
370.641997	22722.686024	29.545728
370.760260	22772.263301	29.550746
371.456833	22798.054329	29.555764
371.910135	22833.567851	29.560781
372.333372	22867.180229	29.565799
372.746558	22910.750983	29.570816
373.243733	22948.822737	29.575834
374.037948	22980.400064	29.580852
373.983772	23018.499993	29.585869
373.937235	23052.054753	29.590887
374.960076	23092.439698	29.595904
375.014364	23133.336348	29.600922
375.655548	23167.337449	29.605940
376.078835	23201.210639	29.610957
376.642994	23227.768401	29.615975
377.289855	23257.492746	29.620992
377.054708	23292.077192	29.626010
377.628496	23323.865015	29.631028
378.431853	23357.921697	29.636045
378.098529	23387.699406	29.641063
378.457789	23416.646924	29.646080
378.737305	23452.649283	29.651098
379.063886	23500.431512	29.656116
379.217601	23542.006483	29.661133
379.800860	23574.955262	29.666151
380.433455	23623.598635	29.671168
380.712779	23675.077145	29.676186
381.027261	23706.364551	29.681204
381.367889	23754.763261	29.686221
381.663437	23785.658179	29.691239
382.313688	23828.173557	29.696256
382.467695	23888.326637	29.701274
382.643057	23923.153598	29.706292
383.587598	23959.696799	29.711309
383.771289	24001.083463	29.716327
384.400038	24030.170416	29.721344
384.408637	24078.139255	29.726362
384.777692	24102.494758	29.731380
385.355054	24161.028894	29.736397
385.871219	24199.631706	29.741415
386.282006	24232.031577	29.746432
386.313632	24281.066249	29.751450
386.462141	24315.838534	29.756468
387.328730	24355.631058	29.761485
387.468033	24408.987669	29.766503
388.062226	24441.557897	29.771520
388.506882	24498.713337	29.776538
388.951752	24529.022020	29.781556
389.392396	24576.600799	29.786573
389.266854	24615.439866	29.791591
389.932329	24650.759741	29.796608
390.331196	24690.529402	29.801626
390.584106	24730.922467	29.806644
390.857914	24779.281525	29.811661
391.368948	24818.656091	29.816679
391.517773	24868.939303	29.821696
391.845460	24914.609202	29.826714
392.685258	24958.444312	29.831732
393.025016	25008.521363	29.836749
393.228232	25053.102086	29.841767
393.946291	25080.047318	29.846784
394.189570	25123.694409	29.851802
394.438640	25159.367968	29.856820
394.969325	25204.782772	29.861837
395.298915	25240.550427	29.866855
396.143135	25251.345158	29.871872
396.546319	25285.717824	29.876890
397.135892	25317.188250	29.881908
397.788290	25340.888466	29.886925
397.997757	25377.606620	29.891943
398.721839	25394.339382	29.896960
399.138272	25423.988908	29.901978
399.586954	25469.821652	29.906996
399.877917	25484.383695	29.912013
400.301413	25501.899480	29.917031
400.989954	25524.392378	29.922048
401.316559	25558.150635	29.927066
401.630534	25575.407052	29.932084
402.045822	25600.890868	29.937101
402.230194	25632.969699	29.942119
402.759764	25653.584111	29.947136
402.540562	25694.483221	29.952154
402.988561	25729.219957	29.957172
403.495045	25759.886502	29.962189
403.830814	25795.269531	29.967207
404.306422	25835.005535	29.972224
404.545385	25873.872406	29.977242
405.092804	25906.450014	29.982260
405.278863	25942.531435	29.987277
405.315826	25978.057244	29.992295
405.953652	26018.132728	29.997312
406.223994	26070.988769	30.002330
406.377111	26115.591583	30.007348
406.857356	26151.990702	30.012365
407.221629	26214.675103	30.017383
407.645796	26255.975479	30.022400
407.941352	26310.269450	30.027418
408.338283	26364.550001	30.032436
408.645629	26418.561663	30.037453
408.913294	26457.901371	30.042471
409.231415	26515.567035	30.047488
410.288144	26563.765542	30.052506
410.652661	26610.432139	30.057524
411.454777	26655.414864	30.062541
411.781738	26696.498963	30.067559
412.531036	26727.060898	30.072576
412.620241	26780.289686	30.077594
412.768642	26824.217002	30.082612
413.331846	26859.134129	30.087629
413.475098	26917.577547	30.092647
413.906461	26957.269846	30.097664
414.181805	27003.529596	30.102682
415.039563	27047.343453	30.107700
415.056594	27099.168961	30.112717
415.348181	27147.990706	30.117735
416.334269	27189.326670	30.122752
416.546600	27241.404215	30.127770
417.175762	27280.932114	30.132788
417.997165	27325.351974	30.137805
418.150391	27373.165809	30.142823
418.753980	27411.972778	30.147840
419.100398	27460.839975	30.152858
419.201690	27495.762158	30.157876
419.353029	27537.167464	30.162893
419.912866	27590.488185	30.167911
420.361884	27628.551552	30.172928
420.594394	27670.842719	30.177946
421.179060	27714.999891	30.182964
421.694611	27745.444545	30.187981
421.716812	27784.165451	30.192999
422.148119	27830.051538	30.198016
422.506835	27881.236265	30.203034
423.114510	27918.993337	30.208052
423.451765	27965.295912	30.213069
423.897387	28027.702221	30.218087
424.592253	28063.464319	30.223104
424.702431	28105.388784	30.228122
424.723350	28154.365340	30.233140
425.614131	28209.607901	30.238157
425.770035	28259.931429	30.243175
426.294909	28297.851263	30.248192
426.954538	28343.063823	30.253210
427.703798	28373.953595	30.258228
428.363962	28418.365062	30.263245
428.541105	28473.436156	30.268263
429.051405	28501.003083	30.273280
429.378577	28548.059626	30.278298
429.746808	28598.759134	30.283316
430.176305	28634.156184	30.288333
430.272531	28693.550242	30.293351
430.773841	28740.982306	30.298368
431.293693	28787.335781	30.303386
431.926076	28840.295086	30.308404
432.537944	28884.542237	30.313421
432.598100	28938.489075	30.318439
432.964308	28976.922394	30.323456
433.872851	29028.820924	30.328474
433.830516	29077.895712	30.333492
434.311443	29127.616040	30.338509
434.500755	29182.482336	30.343527
435.045233	29228.627882	30.348544
435.440149	29277.280855	30.353562
435.800565	29342.403085	30.358580
436.476945	29386.432662	30.363597
436.618909	29438.875451	30.368615
437.211560	29507.152326	30.373632
437.661589	29549.355370	30.378650
438.234246	29597.579251	30.383668
439.068913	29649.084904	30.388685
439.041799	29694.278793	30.393703
439.420255	29749.983146	30.398720
440.064807	29805.656339	30.403738
440.766068	29846.705031	30.408756
441.469190	29892.450738	30.413773
441.800496	29949.270790	30.418791
442.709784	29982.695405	30.423808
442.972230	30015.009247	30.428826
443.120539	30069.676910	30.433844
444.051485	30107.864867	30.438861
444.308740	30143.731949	30.443879
444.460763	30190.856581	30.448896
444.964100	30229.213235	30.453914
445.665793	30269.000983	30.458932
445.973790	30313.513338	30.463949
445.718257	30367.819609	30.468967
446.462914	30405.338648	30.473984
447.229923	30449.280236	30.479002
447.090044	30513.145582	30.484020
447.823171	30554.077110	30.489037
447.899514	30611.007686	30.494055
448.454668	30660.392042	30.499072
449.061807	30709.345211	30.504090
449.248895	30762.017981	30.509108
449.640152	30810.675845	30.514125
449.741809	30874.174512	30.519143
450.645904	30900.191138	30.524160
451.205693	30959.831833	30.529178
451.444655	31016.721093	30.534196
452.046746	31058.792259	30.539213
452.448634	31097.429433	30.544231
452.878520	31152.315823	30.549248
453.588165	31195.136177	30.554266
454.083046	31247.469319	30.559284
454.592316	31283.439081	30.564301
454.718143	31337.019684	30.569319
455.232886	31392.997019	30.574336
455.961258	31439.591282	30.579354
456.028200	31493.510200	30.584372
456.312025	31544.784341	30.589389
456.803432	31597.598650	30.594407
457.441806	31639.242458	30.599424
457.235347	31707.417020	30.604442
457.822098	31761.414951	30.609460
458.836637	31810.884419	30.614477
459.260848	31876.475656	30.619495
459.555387	31922.398293	30.624512
460.136404	31982.379702	30.629530
460.261821	32041.067304	30.634548
461.276857	32090.288234	30.639565
462.009959	32146.225593	30.644583
462.555806	32193.801675	30.649600
463.185828	32246.058683	30.654618
463.327635	32287.271786	30.659636
464.263875	32329.287652	30.664653
464.459189	32381.998634	30.669671
464.684988	32438.721150	30.674688
465.234246	32478.106862	30.679706
465.951722	32529.769732	30.684724
466.280054	32574.073082	30.689741
466.710301	32624.155644	30.694759
467.399209	32659.801976	30.699776
468.066819	32719.086936	30.704794
468.198169	32778.549022	30.709812
468.835314	32809.335832	30.714829
469.172697	32858.320634	30.719847
469.257465	32909.224622	30.724864
469.784245	32954.392213	30.729882
470.293948	33017.443136	30.734900
470.581382	33066.329491	30.739917
471.015571	33122.609609	30.744935
471.086518	33188.699507	30.749952
472.152387	33238.069862	30.754970
472.074984	33303.500012	30.759988
472.924124	33368.685849	30.765005
473.154841	33428.209434	30.770023
473.737243	33490.808303	30.775040
474.382939	33537.932940	30.780058
473.930205	33608.774405	30.785076
474.593856	33660.351665	30.790093
474.976247	33727.180952	30.795111
475.658134	33802.139604	30.800128
476.335275	33862.389202	30.805146
476.455728	33935.977089	30.810164
477.104383	33998.301759	30.815181
477.603833	34057.420202	30.820199
478.217673	34125.014219	30.825216
478.703652	34189.518402	30.830234
479.209923	34237.030801	30.835252
479.516288	34313.063373	30.840269
480.110342	34388.903598	30.845287
480.935084	34437.559834	30.850304
481.602532	34493.663785	30.855322
482.038953	34555.246077	30.860340
482.639295	34598.550309	30.865357
482.919752	34645.413212	30.870375
483.407414	34700.995309	30.875392
484.308589	34751.233297	30.880410
484.537061	34787.326017	30.885428
484.907990	34846.938488	30.890445
485.186698	34906.052042	30.895463
485.596332	34956.109897	30.900480
486.129706	35020.473579	30.905498
486.302361	35073.186848	30.910516
486.983539	35144.339387	30.915533
487.521612	35218.381108	30.920551
487.808038	35270.605986	30.925568
488.383273	35330.877400	30.930586
488.548609	35400.440552	30.935604
489.096994	35468.940371	30.940621
489.616492	35513.093265	30.945639
489.938641	35591.148285	30.950656
491.509637	35647.371698	30.955674
491.590424	35708.489728	30.960692
492.261324	35761.671813	30.965709
492.770679	35817.531509	30.970727
492.933781	35868.421566	30.975744
493.667887	35933.780985	30.980762
494.209152	36000.624124	30.985780
494.724966	36063.337722	30.990797
495.348428	36123.976223	30.995815
495.602406	36176.616199	31.000832
496.520363	36234.634501	31.005850
496.985733	36297.035365	31.010868
497.633493	36341.339531	31.015885
498.294120	36391.258966	31.020903
498.719983	36441.087932	31.025920
499.351792	36497.257725	31.030938
499.805982	36558.541039	31.035956
500.111705	36594.517353	31.040973
500.720697	36648.968317	31.045991
501.045452	36720.075552	31.051008
501.734742	36764.007828	31.056026
501.872682	36828.730524	31.061044
502.868459	36873.799045	31.066061
503.056083	36918.095436	31.071079
503.234353	36989.357324	31.076096
503.934058	37048.547277	31.081114
504.132650	37108.530278	31.086132
504.703973	37175.783101	31.091149
505.026844	37232.009381	31.096167
505.381315	37302.242975	31.101184
506.255465	37351.242993	31.106202
506.880595	37431.973250	31.111220
507.246314	37491.409186	31.116237
507.566575	37544.402004	31.121255
508.278409	37611.150379	31.126272
509.129538	37680.981501	31.131290
509.073968	37738.108213	31.136308
509.643263	37789.911827	31.141325
510.346871	37873.616698	31.146343
510.713635	37933.401083	31.151360
511.798866	37994.622927	31.156378
512.100340	38053.386463	31.161396
512.792496	38105.524170	31.166413
513.454192	38149.764219	31.171431
513.572248	38200.655694	31.176448
514.169297	38263.208901	31.181466
514.786015	38326.188308	31.186484
515.253900	38379.907194	31.191501
515.673067	38430.519181	31.196519
516.036269	38492.202841	31.201536
516.921681	38550.458084	31.206554
517.285109	38586.375191	31.211572
517.854050	38639.080807	31.216589
518.644173	38689.316628	31.221607
519.226012	38744.078249	31.226624
519.723756	38786.481631	31.231642
519.655298	38851.138360	31.236660
520.150394	38893.078466	31.241677
520.801678	38937.148571	31.246695
520.827662	39013.682931	31.251712
521.493373	39070.921957	31.256730
521.584714	39129.357571	31.261748
522.179549	39214.024020	31.266765
523.014974	39276.099475	31.271783
522.999988	39352.818782	31.276800
523.912087	39405.883421	31.281818
524.725926	39474.130539	31.286836
525.634627	39521.644119	31.291853
526.103636	39586.666042	31.296871
526.519993	39643.979626	31.301888
527.292532	39705.571392	31.306906
527.542299	39770.276672	31.311924
528.245644	39838.032077	31.316941
528.654800	39894.912061	31.321959
528.449139	39969.765316	31.326976
528.801154	40045.568380	31.331994
529.328198	40107.760742	31.337012
529.745869	40188.850040	31.342029
530.151572	40267.599586	31.347047
530.412753	40358.042806	31.352064
530.968167	40442.996095	31.357082
531.405355	40522.189758	31.362100
532.034898	40614.628284	31.367117
532.926684	40692.794331	31.372135
533.452508	40777.810881	31.377152
534.101961	40859.448830	31.382170
534.524653	40937.589241	31.387188
535.283904	41016.176291	31.392205
535.605411	41089.927476	31.397223
536.279441	41185.843264	31.402240
537.169819	41262.342131	31.407258
537.917331	41338.902795	31.412276
538.232277	41406.769210	31.417293
539.453555	41468.965171	31.422311
540.089957	41543.704711	31.427328
540.642089	41601.696477	31.432346
541.116849	41666.074572	31.437364
541.712945	41724.798133	31.442381
542.289762	41791.622040	31.447399
542.675895	41863.610527	31.452416
543.396222	41923.497976	31.457434
544.140630	41978.097247	31.462452
544.496484	42037.745379	31.467469
545.541810	42105.563184	31.472487
546.167514	42156.561777	31.477504
547.001432	42198.245168	31.482522
547.553082	42247.245372	31.487540
547.745080	42302.441938	31.492557
548.280454	42346.195330	31.497575
548.640107	42413.379362	31.502592
549.144878	42476.473668	31.507610
549.513398	42538.864620	31.512628
549.923779	42595.096160	31.517645
550.651109	42661.380642	31.522663
550.735423	42732.737338	31.527680
551.586017	42797.499276	31.532698
551.658097	42862.759389	31.537716
551.921496	42928.471137	31.542733
552.883650	42979.536399	31.547751
553.000481	43056.975518	31.552768
553.510251	43117.476190	31.557786
553.905218	43186.841807	31.562804
554.366459	43262.169719	31.567821
554.829607	43340.689330	31.572839
555.130929	43422.696069	31.577856
555.877403	43493.766380	31.582874
556.377466	43585.786613	31.587892
556.601713	43664.283914	31.592909
557.372580	43738.716536	31.597927
557.676362	43835.240808	31.602944
558.725210	43899.298247	31.607962
559.087760	43995.886259	31.612980
559.322829	44071.750480	31.617997
560.199907	44161.886490	31.623015
560.506445	44250.885892	31.628032
561.427489	44330.246471	31.633050
561.963920	44414.864448	31.638068
562.792092	44499.137849	31.643085
563.461764	44570.171296	31.648103
564.209053	44650.307037	31.653120
564.743620	44732.486249	31.658138
565.254309	44807.973281	31.663156
565.820594	44890.094276	31.668173
566.475750	44958.665795	31.673191
566.647359	45055.192964	31.678208
567.419607	45130.492866	31.683226
568.119850	45219.548683	31.688244
568.721775	45288.319644	31.693261
569.809869	45354.459440	31.698279
570.920760	45419.983184	31.703296
571.405193	45489.371028	31.708314
572.260108	45556.399381	31.713332
572.461669	45617.315876	31.718349
573.151403	45682.335462	31.723367
573.293319	45761.474040	31.728384
574.116774	45817.470290	31.733402
574.919092	45891.262211	31.738420
574.928196	45960.133559	31.743437
575.939676	46028.350194	31.748455
576.621409	46105.516074	31.753472
577.055676	46163.427906	31.758490
577.796720	46227.370532	31.763508
578.268262	46303.204758	31.768525
578.873058	46352.488030	31.773543
579.001019	46423.182261	31.778560
579.741769	46501.663015	31.783578
580.558151	46570.188551	31.788596
580.897358	46648.635201	31.793613
581.957760	46708.222991	31.798631
582.151308	46786.902674	31.803648
582.632004	46852.409218	31.808666
583.718923	46922.394360	31.813684
583.977285	46984.471057	31.818701
584.947881	47052.164535	31.823719
586.031872	47114.771550	31.828736
586.420094	47175.131786	31.833754
586.828954	47235.103574	31.838772
587.040531	47296.557499	31.843789
587.854939	47355.332248	31.848807
588.358814	47426.864932	31.853824
588.734348	47497.819125	31.858842
589.203672	47563.787884	31.863860
589.677010	47640.476618	31.868877
590.302136	47709.745218	31.873895
591.103274	47773.452660	31.878912
591.592474	47834.436187	31.883930
591.871929	47903.137356	31.888948
591.905311	47966.593327	31.893965
592.687108	48033.857322	31.898983
593.313959	48116.051888	31.904000
593.602200	48192.726066	31.909018
594.429035	48258.805563	31.914036
594.970798	48338.728895	31.919053
595.776076	48406.119806	31.924071
596.371045	48491.359102	31.929088
596.662130	48557.013398	31.934106
597.567568	48646.108382	31.939124
597.435954	48730.432975	31.944141
598.300656	48798.693358	31.949159
599.240348	48897.345983	31.954176
599.496938	48972.872742	31.959194
600.185205	49044.940033	31.964212
600.640665	49127.650453	31.969229
601.533398	49201.468810	31.974247
601.707382	49298.156251	31.979264
602.741091	49379.360640	31.984282
603.450244	49453.728208	31.989300
603.972865	49544.463317	31.994317
604.850140	49626.531473	31.999335
605.314209	49718.941368	32.004352
606.176065	49794.140874	32.009370
607.006301	49863.651891	32.014388
607.479882	49943.580593	32.019405
608.487641	50005.916055	32.024423
608.458110	50081.017585	32.029440
609.318145	50167.003813	32.034458
610.420124	50238.138801	32.039476
610.851777	50318.723415	32.044493
611.741076	50402.315149	32.049511
611.840758	50473.025977	32.054528
612.768512	50545.567849	32.059546
613.251815	50617.355954	32.064564
613.500870	50700.337823	32.069581
613.896067	50770.404036	32.074599
614.283126	50860.962494	32.079616
615.431465	50952.962139	32.084634
615.942195	51027.374916	32.089652
616.465990	51124.080127	32.094669
617.137553	51199.171304	32.099687
617.899687	51286.502050	32.104704
618.258452	51368.259050	32.109722
618.608475	51457.661015	32.114740
619.023876	51561.947389	32.119757
619.912690	51640.908135	32.124775
620.258940	51736.353973	32.129792
620.908825	51831.993331	32.134810
621.480954	51919.026695	32.139828
621.747635	52024.616133	32.144845
622.419468	52121.898844	32.149863
623.101162	52213.526771	32.154880
623.856099	52324.292884	32.159898
624.119558	52419.888429	32.164916
624.966314	52524.851006	32.169933
625.747445	52610.987535	32.174951
626.581661	52713.198971	32.179968
627.351993	52803.387392	32.184986
628.174644	52896.568235	32.190004
628.651075	52999.010834	32.195021
629.516824	53078.275012	32.200039
630.464840	53177.576824	32.205056
630.961288	53261.703845	32.210074
631.873602	53331.731850	32.215092
632.153337	53435.340031	32.220109
632.476924	53502.755757	32.225127
633.088029	53582.335697	32.230144
634.216275	53663.384630	32.235162
635.019914	53748.619107	32.240180
635.209301	53821.882766	32.245197
636.192626	53884.863404	32.250215
637.168346	53961.137497	32.255232
637.815059	54042.330715	32.260250
638.727417	54100.989959	32.265268
639.162740	54180.784586	32.270285
639.785889	54242.638168	32.275303
640.242950	54319.751119	32.280320
640.902960	54403.704439	32.285338
641.384546	54466.870909	32.290356
642.132516	54542.079301	32.295373
642.512870	54624.670916	32.300391
643.083842	54708.621299	32.305408
643.370308	54783.022357	32.310426
644.032629	54875.019824	32.315444
644.596806	54973.117988	32.320461
645.099140	55057.523450	32.325479
646.005487	55149.684075	32.330496
646.355199	55253.429335	32.335514
646.918979	55331.975449	32.340532
647.306198	55437.155974	32.345549
648.563903	55533.006925	32.350567
649.221649	55622.209780	32.355584
649.534227	55711.324732	32.360602
650.515423	55810.002647	32.365620
651.142053	55892.261974	32.370637
652.249500	55991.419080	32.375655
653.063135	56079.581043	32.380672
653.638450	56164.377251	32.385690
654.106262	56248.155390	32.390708
655.147665	56338.087906	32.395725
655.475549	56413.158030	32.400743
656.070560	56515.984873	32.405760
656.435564	56610.206746	32.410778
657.308006	56703.580738	32.415796
657.797001	56791.136069	32.420813
658.588629	56891.398716	32.425831
659.229823	56994.062459	32.430848
659.642605	57074.169525	32.435866
660.660459	57160.944115	32.440884
661.115351	57269.295128	32.445901
661.874429	57366.399963	32.450919
662.907576	57452.914245	32.455936
663.986741	57541.108382	32.460954
664.924134	57601.606355	32.465972
665.296868	57697.437062	32.470989
666.000143	57769.632197	32.476007
666.956062	57853.785149	32.481024
667.260259	57944.295352	32.486042
667.699945	58018.411597	32.491060
668.028754	58101.727669	32.496077
668.787271	58195.253881	32.501095
669.599957	58295.393771	32.506112
669.628380	58411.239806	32.511130
670.539968	58487.358784	32.516148
670.814382	58593.073906	32.521165
671.381972	58689.679716	32.526183
672.573289	58780.925548	32.531200
673.171632	58883.454470	32.536218
673.827500	58973.266718	32.541236
674.353833	59080.054972	32.546253
675.140038	59183.704488	32.551271
676.052020	59281.368454	32.556288
676.139675	59379.674573	32.561306
676.678179	59471.075606	32.566324
677.344002	59574.323636	32.571341
678.376238	59653.093868	32.576359
679.114691	59734.516493	32.581376
679.370427	59837.820968	32.586394
680.783100	59924.839405	32.591412
681.764213	60013.382960	32.596429
682.411646	60079.693332	32.601447
683.557603	60172.235848	32.606464
684.009276	60255.799695	32.611482
684.867167	60328.237641	32.616500
685.744095	60421.628315	32.621517
685.935441	60491.876615	32.626535
686.811196	60575.845721	32.631552
687.124663	60670.310142	32.636570
687.923075	60760.049970	32.641588
687.978462	60846.746747	32.646605
688.520986	60936.447464	32.651623
689.333204	61043.224214	32.656640
689.643371	61157.586019	32.661658
690.159093	61251.722726	32.666676
690.922038	61364.645846	32.671693
691.394812	61481.276729	32.676711
692.140191	61573.114486	32.681728
692.845918	61697.500589	32.686746
694.220237	61796.547670	32.691764
694.927703	61896.539609	32.696781
695.399536	62008.850795	32.701799
696.405810	62106.967930	32.706816
697.075515	62202.549881	32.711834
697.931209	62298.120525	32.716852
698.519066	62409.972359	32.721869
699.179623	62512.383060	32.726887
700.259565	62602.350004	32.731904
700.742534	62709.986256	32.736922
701.484250	62814.009378	32.741940
702.034304	62923.759298	32.746957
702.596076	63023.123522	32.751975
703.639158	63129.108355	32.756992
704.230546	63243.169994	32.762010
704.991133	63332.238518	32.767028
705.642944	63454.830294	32.772045
705.716685	63560.490772	32.777063
706.418332	63658.337019	32.782080
707.163979	63777.584298	32.787098
707.808205	63902.556549	32.792116
708.323532	64014.523956	32.797133
709.046774	64129.466289	32.802151
709.926737	64253.219774	32.807168
710.847724	64366.221913	32.812186
711.738719	64481.441910	32.817204
712.190463	64593.536747	32.822221
712.939795	64704.843506	32.827239
714.009545	64808.961644	32.832256
714.575863	64938.017402	32.837274
715.117077	65038.500948	32.842292
716.186707	65138.341470	32.847309
716.797147	65251.797980	32.852327
717.750892	65357.025265	32.857344
718.428655	65476.413703	32.862362
719.264644	65589.057320	32.867380
720.362560	65688.358533	32.872397
721.000553	65796.604834	32.877415
721.440419	65890.712198	32.882432
721.816565	66023.080538	32.887450
722.244201	66128.676769	32.892468
722.929404	66240.027673	32.897485
723.206915	66376.769964	32.902503
723.870305	66471.538400	32.907520
724.190773	66593.798986	32.912538
725.294937	66714.755071	32.917556
726.071428	66831.454692	32.922573
726.824026	66945.769363	32.927591
727.406352	67066.984356	32.932608
728.148776	67188.717273	32.937626
728.630912	67297.281601	32.942644
729.238792	67438.401466	32.947661
729.789890	67567.071492	32.952679
730.847279	67676.491053	32.957696
731.605910	67812.448939	32.962714
732.370469	67932.387137	32.967732
733.716126	68057.306538	32.972749
734.168745	68184.359252	32.977767
735.456247	68289.799132	32.982784
736.052120	68423.372871	32.987802
736.849466	68534.824971	32.992820
737.773759	68655.885216	32.997837
738.213386	68776.058916	33.002855
739.605387	68879.524648	33.007872
739.802818	69002.812200	33.012890
740.823340	69115.507602	33.017908
741.319533	69229.105766	33.022925
742.382383	69347.188295	33.027943
743.082462	69471.059415	33.032960
743.452485	69589.257713	33.037978
744.004569	69707.711113	33.042996
744.988447	69832.890479	33.048013
745.252721	69966.383339	33.053031
746.335877	70086.255904	33.058048
746.902778	70218.631873	33.063066
747.617864	70349.428842	33.068084
748.491667	70469.255952	33.073101
749.268101	70618.582371	33.078119
750.063920	70746.232412	33.083136
750.721746	70866.913061	33.088154
751.288237	70997.536231	33.093172
752.399512	71129.486546	33.098189
753.165474	71244.581080	33.103207
754.150044	71384.501721	33.108224
754.402610	71507.895892	33.113242
754.859207	71638.958452	33.118260
756.136633	71776.911121	33.123277
756.800849	71919.986445	33.128295
757.761173	72046.548508	33.133312
758.590567	72168.725725	33.138330
759.798081	72293.648679	33.143348
760.157448	72431.908935	33.148365
760.547152	72555.438252	33.153383
761.749029	72674.831528	33.158400
762.397104	72815.013109	33.163418
763.119169	72939.678531	33.168436
763.822004	73069.299062	33.173453
764.390108	73223.028556	33.178471
765.336488	73329.789186	33.183488
766.175228	73463.019310	33.188506
766.721558	73606.827241	33.193524
767.841876	73731.659125	33.198541
768.340502	73874.553473	33.203559
769.514194	74008.876226	33.208576
770.202128	74147.346170	33.213594
770.996975	74263.830678	33.218612
772.034922	74387.453145	33.223629
772.072960	74524.394963	33.228647
773.152415	74643.123728	33.233664
773.850796	74783.252854	33.238682
774.207291	74912.789851	33.243700
775.417852	75043.862431	33.248717
776.080360	75160.670829	33.253735
776.887221	75286.714398	33.258752
777.792209	75411.458705	33.263770
778.446817	75529.041919	33.268788
778.980243	75648.903495	33.273805
779.532407	75782.669492	33.278823
780.163058	75911.092035	33.283840
781.042205	76047.468149	33.288858
782.088957	76187.333743	33.293876
782.847632	76312.588003	33.298893
783.760277	76442.927640	33.303911
784.637351	76580.395207	33.308928
785.111897	76720.782430	33.313946
785.907906	76847.646313	33.318964
786.613894	76984.676650	33.323981
786.951543	77134.651801	33.328999
787.787754	77275.109329	33.334016
789.110885	77406.240716	33.339034
789.888120	77548.607120	33.344052
791.169885	77683.807436	33.349069
791.537824	77828.760475	33.354087
792.463591	77972.142342	33.359104
793.405052	78113.062183	33.364122
793.697819	78246.961897	33.369140
794.730748	78392.049157	33.374157
795.270084	78545.346458	33.379175
796.148264	78684.129890	33.384192
797.225555	78820.022388	33.389210
798.343498	78964.024091	33.394228
799.396800	79088.385236	33.399245
799.798260	79238.496923	33.404263
800.344688	79388.130266	33.409280
801.399128	79517.838422	33.414298
801.988430	79666.606319	33.419316
802.895306	79812.919141	33.424333
803.380375	79956.367603	33.429351
804.432401	80100.501387	33.434368
805.045468	80252.052434	33.439386
805.938740	80400.503021	33.444404
807.065571	80553.249015	33.449421
807.691907	80700.575443	33.454439
808.619716	80829.167182	33.459456
809.048221	80980.323480	33.464474
809.787965	81137.362905	33.469492
810.924255	81279.668544	33.474509
811.404548	81442.895237	33.479527
812.106223	81591.941996	33.484544
813.355294	81745.409693	33.489562
813.751226	81903.643556	33.494580
814.905100	82045.951123	33.499597
815.496013	82197.974388	33.504615
816.354639	82356.799243	33.509632
817.465872	82517.278887	33.514650
818.096713	82661.378406	33.519668
819.280465	82812.624673	33.524685
820.069865	82964.050937	33.529703
820.822457	83122.702543	33.534720
821.508802	83265.246789	33.539738
822.137725	83418.689031	33.544756
823.447918	83553.224142	33.549773
824.192828	83700.949067	33.554791
824.940528	83852.305872	33.559808
825.829203	83998.376753	33.564826
826.532388	84150.375530	33.569844
827.374231	84316.783356	33.574861
828.142805	84465.382374	33.579879
829.148049	84603.915508	33.584896
830.500663	84747.339600	33.589914
830.896649	84891.472980	33.594932
832.070322	85016.485850	33.599949
832.852812	85145.961129	33.604967
834.106358	85274.486247	33.609984
834.928732	85390.018269	33.615002
835.535913	85517.525289	33.620020
836.799280	85646.588648	33.625037
837.502108	85773.410631	33.630055
838.071425	85899.812464	33.635072
838.926184	86035.057366	33.640090
839.401995	86181.994832	33.645108
839.988264	86317.659017	33.650125
840.798255	86456.330421	33.655143
841.618468	86608.686723	33.660160
842.454960	86731.417150	33.665178
843.252901	86878.913249	33.670196
844.063958	87037.310102	33.675213
844.876482	87184.198303	33.680231
845.562429	87335.056634	33.685248
846.443159	87484.384170	33.690266
847.364931	87651.024232	33.695284
848.101043	87799.612036	33.700301
848.721746	87955.116897	33.705319
849.593000	88098.799394	33.710336
850.951090	88262.574957	33.715354
851.397891	88445.681419	33.720372
852.376523	88591.766389	33.725389
853.201166	88756.424450	33.730407
854.097530	88928.291883	33.735424
855.266064	89070.665667	33.740442
856.167824	89227.967624	33.745460
857.040099	89380.909206	33.750477
857.554456	89546.794693	33.755495
858.329418	89700.868142	33.760512
859.628647	89865.961822	33.765530
860.040793	90029.500862	33.770548
860.853358	90181.755054	33.775565
861.819410	90359.981201	33.780583
862.533779	90536.820054	33.785600
863.544176	90690.506670	33.790618
863.958980	90856.930344	33.795636
865.622957	91016.156034	33.800653
866.564444	91191.740866	33.805671
867.026195	91358.210911	33.810688
868.552913	91510.039248	33.815706
868.489035	91676.338828	33.820724
869.264186	91848.810649	33.825741
870.425261	92015.973527	33.830759
871.719542	92187.286191	33.835776
872.658203	92360.323259	33.840794
873.313922	92529.541397	33.845812
874.125127	92680.526985	33.850829
875.239135	92851.342524	33.855847
875.626775	93022.437433	33.860864
876.987904	93184.619848	33.865882
877.814857	93360.024255	33.870900
878.611111	93522.802203	33.875917
879.707210	93685.620342	33.880935
880.391358	93856.058263	33.885952
881.265046	94024.959736	33.890970
881.939156	94199.958741	33.895988
882.667416	94358.797753	33.901005
883.862488	94537.529718	33.906023
884.727084	94701.886611	33.911040
885.206951	94873.789495	33.916058
886.180054	95059.378706	33.921076
887.020337	95221.641732	33.926093
887.982395	95387.677120	33.931111
888.595817	95557.296778	33.936128
889.279497	95708.955192	33.941146
889.976713	95885.475230	33.946164
891.109149	96060.538467	33.951181
891.808501	96231.832296	33.956199
892.624527	96414.229515	33.961216
893.301921	96583.617814	33.966234
894.133888	96765.521269	33.971252
895.421246	96943.559236	33.976269
896.247152	97136.828668	33.981287
896.955186	97307.913306	33.986304
898.393801	97486.215054	33.991322
898.961260	97677.936197	33.996340
900.010077	97845.701928	34.001357
901.307651	98020.042790	34.006375
901.667320	98220.898945	34.011392
903.031051	98374.379481	34.016410
904.068303	98559.712199	34.021428
905.168500	98739.142300	34.026445
906.243308	98899.099120	34.031463
907.485631	99076.355824	34.036480
908.811467	99236.431614	34.041498
909.374764	99409.757590	34.046516
910.153584	99581.029711	34.051533
911.054861	99753.783143	34.056551
911.825360	99921.323870	34.061568
912.969356	100090.114504	34.066586
913.596446	100275.192083	34.071604
914.494742	100441.835186	34.076621
915.351277	100628.953981	34.081639
915.917120	100810.329367	34.086656
916.643510	100991.514936	34.091674
917.276518	101182.884816	34.096692
918.659489	101372.207667	34.101709
919.634259	101540.713026	34.106727
920.578396	101733.276571	34.111744
921.802183	101918.444882	34.116762
922.167172	102112.860656	34.121780
923.695198	102280.728739	34.126797
924.369016	102477.337565	34.131815
925.295789	102675.495311	34.136832
926.088812	102859.696882	34.141850
927.050274	103057.022429	34.146868
927.916759	103230.387712	34.151885
929.050975	103418.361186	34.156903
929.970798	103610.581951	34.161920
931.889806	103777.363213	34.166938
932.909023	103959.477518	34.171956
934.011792	104131.980397	34.176973
935.063038	104298.699355	34.181991
935.675164	104473.096404	34.187008
936.864326	104646.139310	34.192026
937.353512	104828.993089	34.197044
938.654398	104986.715603	34.202061
939.785552	105156.846128	34.207079
940.324506	105338.796128	34.212096
941.029248	105497.095063	34.217114
941.836427	105680.592507	34.222132
942.286678	105864.340134	34.227149
943.443776	106046.199326	34.232167
944.259231	106240.109465	34.237184
945.328323	106422.960967	34.242202
946.129074	106618.079458	34.247220
947.040115	106799.642549	34.252237
948.141265	106980.377617	34.257255
948.897170	107183.093944	34.262272
949.671636	107354.006850	34.267290
950.588826	107532.141742	34.272308
951.620927	107722.442786	34.277325
952.703289	107912.293612	34.282343
953.677388	108090.030233	34.287360
954.459312	108257.300102	34.292378
955.590164	108447.324063	34.297396
956.229111	108620.357316	34.302413
957.176745	108798.217027	34.307431
958.003525	108985.597231	34.312448
959.100249	109163.143442	34.317466
959.923802	109360.000890	34.322484
960.939967	109549.051012	34.327501
961.922398	109739.108663	34.332519
962.695412	109926.124335	34.337536
963.697689	110109.303552	34.342554
964.489215	110316.800358	34.347572
965.399835	110516.666511	34.352589
966.783896	110720.914628	34.357607
967.278876	110919.623722	34.362624
968.357372	111119.605948	34.367642
969.145589	111334.242520	34.372660
970.413041	111542.252820	34.377677
971.679963	111725.981971	34.382695
972.666972	111941.375874	34.387712
973.855321	112138.649346	34.392730
974.326297	112328.784280	34.397748
975.866117	112531.892893	34.402765
977.222713	112721.770332	34.407783
977.749292	112918.297295	34.412800
979.027273	113128.192747	34.417818
979.773194	113334.111270	34.422836
981.001257	113520.785157	34.427853
981.846029	113727.475712	34.432871
982.545676	113920.446876	34.437888
983.693047	114118.982813	34.442906
984.427538	114317.398318	34.447924
985.439608	114543.880558	34.452941
986.670747	114746.739752	34.457959
987.811881	114949.323910	34.462976
988.648591	115142.952382	34.467994
989.832422	115347.838086	34.473012
990.512346	115556.077053	34.478029
991.937432	115763.257041	34.483047
992.794122	115964.907354	34.488064
994.170313	116156.857482	34.493082
994.889847	116376.979649	34.498100
995.681878	116580.862174	34.503117
997.115682	116776.595148	34.508135
998.444185	116968.355978	34.513152
999.520585	117172.195831	34.518170
1000.479486	117367.035749	34.523188
1001.405933	117568.546657	34.528205
1002.712616	117756.211432	34.533223
1003.581526	117942.175934	34.538240
1004.694758	118141.683565	34.543258
1006.032013	118339.217083	34.548276
1006.542235	118532.555309	34.553293
1007.671772	118723.435925	34.558311
1008.167780	118913.776223	34.563328
1009.248855	119118.668221	34.568346
1010.384578	119328.202748	34.573364
1011.262822	119516.621372	34.578381
1012.581860	119708.161474	34.583399
1013.334587	119920.335702	34.588416
1014.659065	120110.559819	34.593434
1015.943874	120312.778474	34.598452
1016.441898	120519.766047	34.603469
1017.566121	120712.320648	34.608487
1018.294840	120898.986348	34.613504
1018.992193	121082.325873	34.618522
1019.950997	121282.970519	34.623540
1020.483118	121480.835909	34.628557
1021.390686	121673.293256	34.633575
1022.613026	121895.731718	34.638592
1023.313456	122103.723539	34.643610
1024.204392	122306.008402	34.648628
1025.438895	122522.810652	34.653645
1026.444612	122738.118959	34.658663
1026.902883	122957.270168	34.663680
1027.961204	123173.916220	34.668698
1029.061872	123394.599335	34.673716
1029.781221	123629.413416	34.678733
1031.480659	123819.485714	34.683751
1032.653780	124058.549596	34.688768
1033.494873	124277.482632	34.693786
1034.684676	124488.249133	34.698804
1036.017562	124719.143356	34.703821
1037.883050	124920.233347	34.708839
1038.826606	125126.609478	34.713856
1039.752240	125325.411460	34.718874
1041.008816	125542.270143	34.723892
1041.996650	125762.862692	34.728909
1042.995788	125958.475728	34.733927
1044.149817	126185.215874	34.738944
1044.905743	126393.456657	34.743962
1046.211938	126613.990197	34.748980
1046.610179	126840.048912	34.753997
1047.484279	127061.975117	34.759015
1048.436493	127288.630102	34.764032
1049.080137	127520.369310	34.769050
1050.043818	127751.892679	34.774068
1051.291405	127980.747366	34.779085
1052.837545	128219.731963	34.784103
1054.124149	128439.572189	34.789120
1055.374960	128657.417325	34.794138
1057.036019	128895.095409	34.799156
1057.833461	129124.311776	34.804173
1059.321177	129326.912894	34.809191
1060.450354	129538.637065	34.814208
1061.473420	129759.658276	34.819226
1062.209502	129981.907219	34.824244
1062.911817	130198.193331	34.829261
1064.193706	130419.379306	34.834279
1065.283502	130644.933524	34.839296
1065.979849	130859.615442	34.844314
1067.061202	131087.151608	34.849332
1068.014744	131306.547444	34.854349
1069.422933	131533.513192	34.859367
1070.373023	131773.650284	34.864384
1071.561572	132005.726009	34.869402
1072.639786	132220.189391	34.874420
1073.378833	132470.139786	34.879437
1074.625418	132693.844782	34.884455
1075.246093	132925.678744	34.889472
1076.394493	133159.189284	34.894490
1077.706302	133394.930964	34.899508
1078.395298	133639.549358	34.904525
1079.679273	133866.856551	34.909543
1080.785885	134117.114128	34.914560
1082.123452	134350.564109	34.919578
1082.990365	134582.927210	34.924596
1083.898348	134826.098678	34.929613
1085.098254	135051.095554	34.934631
1086.279848	135289.648916	34.939648
1087.299919	135540.058591	34.944666
1088.714517	135770.526957	34.949684
1089.270440	135993.278692	34.954701
1090.351104	136222.778514	34.959719
1091.723904	136451.699261	34.964736
1092.670652	136677.395740	34.969754
1093.524341	136900.205919	34.974772
1094.585006	137142.722916	34.979789
1095.591232	137358.829774	34.984807
1096.898736	137580.580762	34.989824
1097.900827	137826.091801	34.994842
1099.048947	138056.620224	34.999860
1100.099407	138294.278918	35.004877
1100.793368	138533.164579	35.009895
1102.008412	138785.608019	35.014912
1102.851382	139019.210980	35.019930
1104.324472	139272.693187	35.024948
1104.863735	139526.813267	35.029965
1106.417775	139761.774764	35.034983
1107.500291	140029.768429	35.040000
1108.194627	140281.472281	35.045018
1109.782684	140526.589449	35.050036
1110.577443	140795.029745	35.055053
1111.513570	141055.321346	35.060071
1112.941143	141306.632825	35.065088
1114.663025	141561.929675	35.070106
1116.044387	141804.161205	35.075124
1116.992949	142049.762632	35.080141
1118.865342	142289.875102	35.085159
1119.817689	142541.248748	35.090176
1120.920067	142779.792646	35.095194
1122.724767	143013.378457	35.100212
1123.672504	143256.046848	35.105229
1124.872490	143481.759812	35.110247
1125.868847	143737.395466	35.115264
1126.692230	143981.078523	35.120282
1128.018980	144201.639653	35.125300
1128.541264	144464.789695	35.130317
1129.499950	144707.948263	35.135335
1130.845457	144961.620454	35.140352
1131.721192	145221.395454	35.145370
1132.914556	145479.243147	35.150388
1133.291572	145749.401331	35.155405
1134.911287	145991.610006	35.160423
1136.271376	146252.327121	35.165440
1137.427392	146523.795590	35.170458
1138.496275	146768.750900	35.175476
1139.461488	147043.311051	35.180493
1140.655368	147314.931463	35.185511
1141.954880	147561.147653	35.190528
1143.048743	147834.056675	35.195546
1143.941279	148090.095994	35.200564
1145.245524	148371.737561	35.205581
1146.789650	148619.898992	35.210599
1147.903317	148899.952814	35.215616
1148.764052	149156.778529	35.220634
1150.184712	149419.778719	35.225652
1150.808415	149693.514910	35.230669
1151.895098	149965.933827	35.235687
1153.390486	150228.559691	35.240704
1154.000590	150505.665082	35.245722
1155.163731	150776.365198	35.250740
1156.231552	151048.351323	35.255757
1157.500617	151335.703432	35.260775
1158.572981	151619.944812	35.265792
1159.527032	151898.716047	35.270810
1160.574430	152189.256764	35.275828
1161.584009	152480.186478	35.280845
1162.732711	152756.002081	35.285863
1164.545518	153033.828240	35.290880
1165.228610	153302.482351	35.295898
1166.415680	153579.147436	35.300916
1167.897016	153842.346407	35.305933
1169.008266	154110.352095	35.310951
1169.967623	154382.646583	35.315968
1171.208633	154661.073699	35.320986
1172.374435	154922.746675	35.326004
1173.519099	155203.375315	35.331021
1174.402800	155487.892456	35.336039
1175.700588	155765.709329	35.341056
1176.612545	156041.080330	35.346074
1177.801600	156333.278194	35.351092
1178.957320	156634.084045	35.356109
1179.761588	156920.971466	35.361127
1180.919054	157213.536297	35.366144
1181.827644	157519.844280	35.371162
1183.625180	157810.582718	35.376180
1184.401989	158120.570444	35.381197
1185.522505	158417.387173	35.386215
1187.034958	158717.909003	35.391232
1188.434928	159023.056526	35.396250
1189.704780	159317.305497	35.401268
1190.728711	159616.062604	35.406285
1192.120278	159933.117670	35.411303
1193.345491	160227.114253	35.416320
1194.670070	160520.589126	35.421338
1195.961037	160833.126240	35.426356
1197.225803	161140.570209	35.431373
1198.412057	161441.546736	35.436391
1199.812861	161733.241659	35.441408
1201.052462	162049.475595	35.446426
1202.078681	162349.800110	35.451444
1203.518718	162650.933879	35.456461
1204.323735	162956.602341	35.461479
1205.575971	163259.458858	35.466496
1206.500852	163572.914481	35.471514
1208.007124	163885.160017	35.476532
1209.099711	164190.384032	35.481549
1210.300141	164504.739966	35.486567
1212.103091	164813.771590	35.491584
1212.922244	165120.113180	35.496602
1214.456679	165425.615715	35.501620
1216.356361	165738.520468	35.506637
1217.624457	166037.676773	35.511655
1218.644540	166349.183264	35.516672
1219.360983	166652.418864	35.521690
1220.808786	166955.396298	35.526708
1222.019172	167273.704161	35.531725
1222.696232	167587.242813	35.536743
1224.309785	167879.224048	35.541760
1225.258513	168210.891896	35.546778
1226.558800	168525.742786	35.551796
1227.937194	168836.167419	35.556813
1228.822229	169138.351931	35.561831
1230.304871	169461.794935	35.566848
1231.133769	169789.218274	35.571866
1232.725882	170098.169898	35.576884
1233.903819	170422.913647	35.581901
1235.138388	170738.983754	35.586919
1236.906657	171045.704895	35.591936
1238.260911	171365.312575	35.596954
1239.519637	171666.691013	35.601972
1241.093203	171978.665882	35.606989
1241.938849	172278.733383	35.612007
1243.602592	172586.103893	35.617024
1244.742186	172891.088480	35.622042
1245.914801	173183.329121	35.627060
1247.352815	173489.676941	35.632077
1248.617450	173791.550471	35.637095
1250.004203	174051.249677	35.642112
1251.156920	174339.084713	35.647130
1252.623229	174622.085566	35.652148
1253.531247	174911.157348	35.657165
1254.395677	175205.466479	35.662183
1255.852889	175499.171971	35.667200
1256.467831	175793.843168	35.672218
1257.918117	176090.522991	35.677236
1259.351885	176392.651635	35.682253
1260.134061	176696.920226	35.687271
1261.760494	176995.835474	35.692288
1262.956443	177316.258433	35.697306
1263.726534	177613.364422	35.702324
1264.912321	177937.080068	35.707341
1266.087698	178255.494688	35.712359
1267.288315	178575.493589	35.717376
1268.138516	178910.426531	35.722394
1269.553209	179235.635831	35.727412
1270.868643	179555.266716	35.732429
1272.023165	179893.189255	35.737447
1273.169371	180235.049820	35.742464
1274.290997	180577.932082	35.747482
1275.893020	180910.913949	35.752500
1276.774532	181243.331550	35.757517
1278.645580	181590.221759	35.762535
1280.385512	181926.373128	35.767552
1281.091784	182273.295182	35.772570
1282.417096	182617.947014	35.777588
1283.853801	182953.063547	35.782605
1284.881087	183304.914833	35.787623
1285.754059	183652.097743	35.792640
1287.008857	184011.214325	35.797658
1288.460571	184376.418661	35.802676
1289.809101	184729.800258	35.807693
1290.847566	185084.517327	35.812711
1292.704418	185444.851512	35.817728
1294.016165	185802.561779	35.822746
1295.462190	186158.259432	35.827764
1296.865060	186512.468736	35.832781
1298.035187	186871.821394	35.837799
1299.636879	187219.351206	35.842816
1300.737833	187582.413631	35.847834
1302.262675	187932.156529	35.852852
1303.730879	188275.602291	35.857869
1305.127742	188636.071313	35.862887
1306.849289	188982.589492	35.867904
1308.509710	189312.859206	35.872922
1310.228110	189646.447038	35.877940
1311.747790	189977.848181	35.882957
1313.233162	190307.733619	35.887975
1314.629550	190627.480408	35.892992
1316.301307	190957.148365	35.898010
1317.567203	191283.254638	35.903028
1318.522784	191600.299484	35.908045
1319.772081	191931.134338	35.913063
1320.959141	192259.797879	35.918080
1321.911309	192590.774305	35.923098
1322.954948	192938.049908	35.928116
1324.189354	193275.356171	35.933133
1325.267854	193629.599327	35.938151
1326.249508	193984.952277	35.943168
1327.463111	194335.381512	35.948186
1328.457878	194684.477816	35.953204
1329.910981	195041.955281	35.958221
1331.492892	195414.482536	35.963239
1332.991362	195759.617072	35.968256
1333.827356	196113.190870	35.973274
1334.888519	196460.953153	35.978292
1336.449701	196803.125054	35.983309
1337.623251	197156.471217	35.988327
1339.127487	197495.545853	35.993344
1340.044519	197845.688104	35.998362
1341.678902	198185.798606	36.003380
1342.816028	198537.050854	36.008397
1343.792530	198896.964576	36.013415
1345.472615	199259.658778	36.018432
1346.797309	199611.977628	36.023450
1347.868586	199971.310219	36.028468
1349.398716	200342.388966	36.033485
1350.559287	200719.358234	36.038503
1351.729830	201080.673622	36.043520
1353.266840	201459.565448	36.048538
1354.374917	201844.014937	36.053556
1355.523415	202221.781616	36.058573
1356.918437	202597.490926	36.063591
1358.774155	202981.163079	36.068608
1360.173947	203365.775927	36.073626
1361.230523	203740.721898	36.078644
1363.651025	204109.718530	36.083661
1365.122777	204484.104691	36.088679
1367.096771	204843.541939	36.093696
1368.244748	205213.706467	36.098714
1369.843279	205574.402773	36.103732
1371.218723	205938.718207	36.108749
1372.150787	206328.553492	36.113767
1373.843513	206671.260537	36.118784
1375.525763	207026.896588	36.123802
1376.739683	207406.126873	36.128820
1378.512646	207766.563655	36.133837
1379.567387	208138.129264	36.138855
1380.806578	208510.605820	36.143872
1382.399892	208865.884115	36.148890
1383.900988	209242.879318	36.153908
1385.354316	209607.326277	36.158925
1386.562040	209983.903598	36.163943
1388.041401	210351.105035	36.168960
1389.288878	210735.272530	36.173978
1390.365787	211092.042676	36.178996
1391.688828	211463.554083	36.184013
1393.500542	211836.776917	36.189031
1394.898576	212210.983947	36.194048
1396.306524	212580.645104	36.199066
1398.087173	212941.281501	36.204084
1399.741618	213329.368278	36.209101
1401.242428	213696.276134	36.214119
1402.505735	214050.018537	36.219136
1403.949866	214432.608513	36.224154
1404.778809	214803.238216	36.229172
1406.399006	215168.151572	36.234189
1407.147536	215550.353218	36.239207
1408.488624	215934.744425	36.244224
1409.642603	216321.834836	36.249242
1411.078387	216712.689963	36.254260
1412.127203	217110.899651	36.259277
1413.218334	217511.999365	36.264295
1414.735345	217905.182637	36.269312
1416.138166	218304.811997	36.274330
1417.612861	218722.793781	36.279348
1419.094845	219110.374838	36.284365
1420.746213	219538.185351	36.289383
1421.861331	219987.141272	36.294400
1423.587376	220385.100277	36.299418
1424.886276	220793.824045	36.304436
1426.406798	221194.639353	36.309453
1427.289502	221606.101873	36.314471
1428.582388	222008.634194	36.319488
1429.842048	222404.061886	36.324506
1431.141706	222813.987182	36.329524
1432.531215	223205.586579	36.334541
1434.059666	223604.377779	36.339559
1435.324517	224014.262542	36.344576
1436.723043	224431.238536	36.349594
1437.766277	224840.451722	36.354612
1439.551784	225260.719619	36.359629
1440.683165	225685.059320	36.364647
1441.708480	226101.848993	36.369664
1444.005578	226530.876102	36.374682
1445.221155	226959.626036	36.379700
1446.467556	227382.352639	36.384717
1448.303989	227799.801743	36.389735
1449.245818	228225.299293	36.394752
1451.213514	228665.437255	36.399770
1452.481198	229091.823749	36.404788
1454.426867	229513.883321	36.409805
1455.745229	229956.647472	36.414823
1457.019030	230384.434188	36.419840
1458.962797	230810.943280	36.424858
1460.652443	231237.673446	36.429876
1462.226069	231667.345152	36.434893
1463.800507	232098.872294	36.439911
1465.091320	232523.208308	36.444928
1466.710536	232955.645063	36.449946
1467.826077	233395.634098	36.454964
1469.645774	233816.762246	36.459981
1471.088734	234252.178365	36.464999
1473.236189	234677.141169	36.470016
1475.071414	235101.902637	36.475034
1476.238647	235533.659233	36.480052
1477.970554	235954.579003	36.485069
1479.457131	236384.329239	36.490087
1481.242155	236799.958880	36.495104
1482.506042	237223.804041	36.500122
1483.672244	237650.993971	36.505140
1484.875002	238073.682797	36.510157
1486.408047	238520.729216	36.515175
1487.810575	238949.178713	36.520192
1489.532801	239375.061647	36.525210
1491.064546	239819.393375	36.530228
1492.396339	240250.575468	36.535245
1493.606199	240687.494079	36.540263
1495.049156	241134.790028	36.545280
1496.278264	241582.858888	36.550298
1497.647559	242030.346708	36.555316
1499.367612	242483.797902	36.560333
1500.589702	242939.186558	36.565351
1502.176680	243402.873285	36.570368
1503.532119	243852.119751	36.575386
1504.462149	244328.592492	36.580404
1506.120563	244771.186002	36.585421
1507.571246	245245.821785	36.590439
1508.836351	245714.138393	36.595456
1510.710508	246184.514530	36.600474
1511.310015	246669.174884	36.605492
1513.487809	247141.991958	36.610509
1514.587055	247624.285169	36.615527
1515.733493	248128.443160	36.620544
1517.440273	248593.058843	36.625562
1518.984266	249096.263611	36.630580
1520.753251	249573.749620	36.635597
1522.260928	250068.985230	36.640615
1523.590669	250550.584036	36.645632
1525.450566	251026.913722	36.650650
1526.848611	251515.488218	36.655668
1528.615776	251987.947602	36.660685
1530.671810	252449.360257	36.665703
1532.020561	252900.017520	36.670720
1534.172340	253368.858328	36.675738
1535.098810	253823.015469	36.680756
1537.125298	254275.238626	36.685773
1538.507079	254747.205162	36.690791
1539.403771	255206.169413	36.695808
1541.291882	255668.907856	36.700826
1542.610633	256140.199794	36.705844
1544.033031	256601.288175	36.710861
1545.855065	257090.051195	36.715879
1546.934990	257579.698981	36.720896
1548.467641	258042.039925	36.725914
1550.084575	258518.415125	36.730932
1552.234335	258996.252129	36.735949
1553.865393	259473.514335	36.740967
1555.124285	259949.415436	36.745984
1557.031524	260436.158426	36.751002
1558.058900	260917.838938	36.756020
1559.943166	261399.708290	36.761037
1561.273840	261906.538786	36.766055
1562.873421	262384.085640	36.771072
1564.827425	262886.672374	36.776090
1565.702160	263386.515684	36.781108
1567.362387	263864.382402	36.786125
1569.366962	264356.392554	36.791143
1571.168149	264859.257838	36.796160
1573.185225	265343.441265	36.801178
1574.399327	265833.015390	36.806196
1576.103085	266320.933423	36.811213
1577.796774	266810.986660	36.816231
1579.383242	267309.186247	36.821248
1580.988195	267806.188438	36.826266
1582.553943	268301.012001	36.831284
1584.325559	268795.572515	36.836301
1586.089194	269271.513404	36.841319
1588.110403	269763.567664	36.846336
1589.785074	270251.817309	36.851354
1591.221771	270739.902441	36.856372
1592.818474	271225.801336	36.861389
1594.883244	271711.469977	36.866407
1595.887181	272211.640258	36.871424
1598.081363	272690.097220	36.876442
1599.688340	273178.760727	36.881460
1601.215919	273654.379575	36.886477
1602.619518	274142.490914	36.891495
1603.749989	274632.272311	36.896512
1605.537170	275114.222126	36.901530
1607.000546	275626.682294	36.906548
1608.421423	276120.503029	36.911565
1609.602057	276627.673409	36.916583
1610.966474	277136.082588	36.921600
1612.778675	277639.310961	36.926618
1614.447076	278141.520515	36.931636
1615.963506	278663.466264	36.936653
1617.537716	279173.360617	36.941671
1619.095282	279691.410647	36.946688
1620.815165	280203.666368	36.951706
1622.936568	280706.760648	36.956724
1624.577257	281213.336876	36.961741
1625.913223	281726.033159	36.966759
1627.471780	282252.840209	36.971776
1628.707462	282764.686606	36.976794
1630.577101	283305.689782	36.981812
1631.873363	283815.364103	36.986829
1633.394185	284348.369358	36.991847
1634.556053	284878.384016	36.996864
1636.114852	285387.324551	37.001882
1637.674245	285918.642006	37.006900
1638.874801	286446.562357	37.011917
1640.638752	286954.702090	37.016935
1642.004191	287486.401924	37.021952
1644.045379	288021.239741	37.026970
1645.182834	288547.842458	37.031988
1646.869765	289090.888557	37.037005
1648.490199	289635.340621	37.042023
1649.852455	290180.646005	37.047040
1651.770106	290725.146397	37.052058
1653.345395	291275.771798	37.057076
1654.728864	291824.724761	37.062093
1656.831227	292374.090224	37.067111
1658.530625	292931.724065	37.072128
1660.408715	293475.000386	37.077146
1661.863496	294045.826835	37.082164
1663.520737	294592.462069	37.087181
1665.356192	295146.710711	37.092199
1667.187412	295717.594142	37.097216
1668.983927	296275.831617	37.102234
1670.658297	296843.077870	37.107252
1672.301034	297406.288037	37.112269
1674.427810	297969.948876	37.117287
1676.095190	298544.553329	37.122304
1677.480379	299099.542664	37.127322
1680.045028	299658.982457	37.132340
1681.696721	300219.966807	37.137357
1683.524512	300778.760205	37.142375
1685.515973	301325.078426	37.147392
1687.656797	301875.915290	37.152410
1689.342713	302415.953845	37.157428
1690.799851	302968.243496	37.162445
1692.438417	303534.265570	37.167463
1693.730407	304096.963605	37.172480
1695.143909	304633.631378	37.177498
1696.363372	305221.223991	37.182516
1697.979402	305793.407631	37.187533
1700.282772	306343.582183	37.192551
1701.490799	306924.613260	37.197568
1703.617686	307499.469951	37.202586
1705.913201	308076.479124	37.207604
1707.250329	308645.845927	37.212621
1709.174708	309223.111784	37.217639
1710.460772	309791.742829	37.222656
1712.499010	310370.480346	37.227674
1713.867721	310949.882951	37.232692
1715.555883	311537.279033	37.237709
1717.580214	312109.530669	37.242727
1718.962384	312700.701766	37.247744
1720.551803	313270.705810	37.252762
1722.428183	313868.465353	37.257780
1724.292614	314454.413851	37.262797
1726.132633	315039.193730	37.267815
1727.979432	315627.421518	37.272832
1729.961236	316192.742616	37.277850
1731.639549	316782.842761	37.282868
1733.173878	317375.475822	37.287885
1735.206213	317952.887544	37.292903
1736.599932	318532.634529	37.297920
1738.298452	319122.458166	37.302938
1740.164430	319712.706266	37.307956
1741.715745	320300.842902	37.312973
1743.489887	320878.552375	37.317991
1744.708068	321482.324511	37.323008
1746.626422	322078.028137	37.328026
1748.931914	322656.853463	37.333044
1750.625827	323238.237545	37.338061
1752.693644	323807.163986	37.343079
1754.290793	324371.415010	37.348096
1755.872846	324925.685093	37.353114
1757.649809	325502.083903	37.358132
1759.202492	326066.200271	37.363149
1761.079474	326626.119507	37.368167
1763.010873	327192.981449	37.373184
1765.338694	327733.088551	37.378202
1767.122874	328301.310144	37.383220
1768.528359	328871.873866	37.388237
1770.213001	329448.301653	37.393255
1771.504142	330027.886145	37.398272
1773.013745	330592.043684	37.403290
1774.459155	331189.566052	37.408308
1776.014087	331786.632599	37.413325
1777.854957	332377.984389	37.418343
1779.110485	332997.149301	37.423360
1780.915635	333607.585243	37.428378
1782.500654	334226.910742	37.433396
1783.802756	334849.957011	37.438413
1785.636745	335473.720838	37.443431
1787.011281	336116.668728	37.448448
1789.161719	336754.150062	37.453466
1791.320742	337395.125543	37.458484
1792.817309	338042.015693	37.463501
1794.983654	338682.593624	37.468519
1796.574709	339327.040852	37.473536
1798.364003	339975.153411	37.478554
1800.027231	340638.229471	37.483572
1802.076163	341283.668161	37.488589
1803.600616	341940.480499	37.493607
1805.385717	342605.668235	37.498624
1807.199213	343270.969317	37.503642
1808.948901	343940.104621	37.508660
1810.306990	344613.838670	37.513677
1812.654613	345287.222481	37.518695
1814.206829	345969.509837	37.523712
1816.349354	346656.537735	37.528730
1818.103936	347324.026328	37.533748
1820.071547	348006.850381	37.538765
1822.283619	348687.517650	37.543783
1824.077646	349372.380646	37.548800
1825.652122	350053.386755	37.553818
1827.688422	350745.016092	37.558836
1829.277594	351435.160588	37.563853
1830.832471	352121.696565	37.568871
1832.631375	352817.875721	37.573888
1834.317861	353513.580321	37.578906
1836.389208	354203.500790	37.583924
1838.554085	354905.955909	37.588941
1840.500631	355594.504589	37.593959
1842.363128	356293.383695	37.598976
1844.145549	356998.709686	37.603994
1846.410548	357687.019812	37.609012
1848.208891	358382.627142	37.614029
1850.306921	359063.482337	37.619047
1852.276629	359761.296563	37.624064
1854.687801	360442.128121	37.629082
1856.767462	361123.916413	37.634100
1858.661002	361798.239349	37.639117
1860.883964	362473.765224	37.644135
1862.670485	363147.804086	37.649152
1864.626028	363806.480005	37.654170
1866.629890	364484.671761	37.659188
1868.267989	365148.629164	37.664205
1870.280708	365804.496878	37.669223
1872.406262	366476.190228	37.674240
1874.183010	367130.526884	37.679258
1876.270551	367767.551069	37.684276
1877.787260	368419.650801	37.689293
1879.624059	369039.064758	37.694311
1881.604976	369669.783527	37.699328
1883.095028	370326.116159	37.704346
1884.919769	370952.704332	37.709364
1886.399290	371598.032902	37.714381
1888.286927	372255.331021	37.719399
1889.878842	372917.916474	37.724416
1891.459231	373568.875155	37.729434
1893.453842	374246.055460	37.734452
1894.692519	374913.506922	37.739469
1896.734542	375589.081489	37.744487
1898.400912	376274.773779	37.749504
1900.200536	376973.694705	37.754522
1901.973193	377661.193780	37.759540
1903.837090	378352.772599	37.764557
1905.740971	379061.956045	37.769575
1907.571128	379770.655207	37.774592
1909.063782	380479.953246	37.779610
1911.308952	381202.019675	37.784628
1912.867079	381927.734065	37.789645
1915.272692	382638.585877	37.794663
1917.194890	383372.373887	37.799680
1918.993909	384099.269167	37.804698
1920.797929	384823.510643	37.809716
1923.070281	385556.964106	37.814733
1925.192762	386281.729268	37.819751
1926.812410	387020.505702	37.824768
1929.115842	387759.405942	37.829786
1931.035963	388493.408615	37.834804
1932.651657	389242.858565	37.839821
1934.936251	389986.096123	37.844839
1936.994111	390724.308728	37.849856
1938.809460	391461.175010	37.854874
1941.366034	392205.481096	37.859892
1943.427274	392935.630220	37.864909
1945.595409	393675.604884	37.869927
1947.676916	394420.670826	37.874944
1949.173001	395154.130070	37.879962
1951.145595	395901.281419	37.884980
1953.069640	396646.901470	37.889997
1955.119467	397391.899250	37.895015
1956.712521	398135.002183	37.900032
1958.400746	398898.269867	37.905050
1960.652746	399655.494442	37.910068
1962.092580	400411.490219	37.915085
1963.755706	401188.209921	37.920103
1966.080490	401961.708012	37.925120
1968.010243	402724.556746	37.930138
1970.351174	403479.360600	37.935156
1972.265872	404266.091477	37.940173
1974.659914	405034.503045	37.945191
1976.278138	405794.128025	37.950208
1978.097521	406571.485896	37.955226
1980.142527	407345.263101	37.960244
1982.117170	408116.243376	37.965261
1984.184287	408898.840931	37.970279
1985.864051	409677.882568	37.975296
1987.722248	410468.829954	37.980314
1989.852067	411245.295113	37.985332
1991.955878	412029.012522	37.990349
1993.965254	412805.629850	37.995367
1996.159847	413592.782229	38.000384
1998.034462	414370.566685	38.005402
2000.625982	415149.577780	38.010420
2002.425556	415927.328675	38.015437
2004.909034	416689.569798	38.020455
2007.064748	417433.632632	38.025472
2009.133338	418183.564128	38.030490
2010.896718	418918.252919	38.035508
2012.520215	419655.729460	38.040525
2014.675388	420407.759583	38.045543
2016.896687	421141.447868	38.050560
2018.150399	421889.227135	38.055578
2020.599268	422644.788740	38.060596
2022.626558	423409.360697	38.065613
2024.615155	424152.671980	38.070631
2027.122755	424898.812458	38.075648
2028.598025	425665.482155	38.080666
2030.902030	426411.028103	38.085684
2033.067432	427182.448239	38.090701
2034.686368	427937.883570	38.095719
2036.888406	428704.287378	38.100736
2038.928701	429488.008747	38.105754
2040.567287	430254.658660	38.110772
2042.321624	431045.514767	38.115789
2044.314549	431828.711605	38.120807
2046.308321	432610.515602	38.125824
2047.912841	433417.718964	38.130842
2050.121386	434224.136900	38.135860
2051.743084	435037.862070	38.140877
2053.641395	435854.094539	38.145895
2056.249693	436664.107462	38.150912
2058.305409	437486.836033	38.155930
2060.341872	438295.417996	38.160948
2062.237810	439117.152668	38.165965
2064.170790	439959.701395	38.170983
2066.412241	440790.376954	38.176000
2068.220588	441638.601821	38.181018
2070.096430	442473.374195	38.186036
2071.822047	443339.207813	38.191053
2073.987396	444189.452444	38.196071
2076.350860	445052.583958	38.201088
2078.144470	445916.433237	38.206106
2080.622993	446768.044181	38.211124
2082.582961	447635.440482	38.216141
2085.001836	448504.294552	38.221159
2087.291365	449368.784621	38.226176
2089.062102	450230.391599	38.231194
2091.423735	451099.655808	38.236212
2093.334879	451964.963032	38.241229
2095.321728	452828.957960	38.246247
2097.849735	453704.359196	38.251264
2099.959674	454570.689766	38.256282
2102.375644	455448.109942	38.261300
2104.366635	456325.209152	38.266317
2106.341964	457205.408826	38.271335
2108.867414	458074.608892	38.276352
2110.309087	458963.720438	38.281370
2112.639681	459834.192405	38.286388
2114.948356	460716.612750	38.291405
2116.962654	461593.633707	38.296423
2119.472138	462469.422605	38.301440
2120.988175	463362.271520	38.306458
2123.394322	464235.017586	38.311476
2125.216391	465123.137102	38.316493
2127.043708	466015.714255	38.321511
2129.254523	466908.339299	38.326528
2131.174840	467813.555853	38.331546
2133.123074	468718.220415	38.336564
2134.827132	469628.542959	38.341581
2137.165131	470528.207393	38.346599
2139.292812	471442.113847	38.351616
2141.127820	472363.149323	38.356634
2143.651300	473252.044489	38.361652
2145.398885	474163.255932	38.366669
2147.650762	475047.210971	38.371687
2150.022466	475918.172172	38.376704
2152.021951	476813.805837	38.381722
2153.899585	477712.194842	38.386740
2156.195779	478616.936756	38.391757
2158.329578	479505.700664	38.396775
2160.696040	480404.080434	38.401792
2162.520681	481312.909225	38.406810
2164.908526	482213.368348	38.411828
2166.296671	483139.247323	38.416845
2168.233581	484056.252790	38.421863
2170.307181	484972.229754	38.426880
2172.370174	485912.094195	38.431898
2174.924317	486855.513873	38.436916
2176.980095	487809.264697	38.441933
2178.922400	488760.004505	38.446951
2181.418460	489715.094498	38.451968
2182.828148	490682.072838	38.456986
2185.405594	491641.940774	38.462004
2187.546130	492608.136798	38.467021
2189.332787	493587.156353	38.472039
2191.629772	494553.520884	38.477056
2193.782492	495550.182948	38.482074
2196.077554	496534.956028	38.487092
2198.305739	497529.774636	38.492109
2200.280819	498525.686707	38.497127
2202.528622	499526.237544	38.502144
2204.817387	500540.141271	38.507162
2207.358772	501536.135076	38.512180
2210.016259	502536.590065	38.517197
2211.985704	503547.337333	38.522215
2214.930862	504524.019755	38.527232
2217.101557	505528.963800	38.532250
2219.809806	506533.606396	38.537268
2221.858304	507533.505525	38.542285
2224.066832	508541.485408	38.547303
2226.339566	509538.198763	38.552320
2228.508181	510545.656970	38.557338
2230.642087	511549.327139	38.562356
2233.107435	512553.182190	38.567373
2235.216254	513561.922332	38.572391
2237.933335	514565.457660	38.577408
2239.864112	515570.772571	38.582426
2242.301565	516569.640028	38.587444
2244.959324	517577.176189	38.592461
2247.473043	518582.353094	38.597479
2250.366372	519572.386792	38.602496
2252.686020	520557.111008	38.607514
2255.262438	521534.172791	38.612532
2257.624035	522518.160116	38.617549
2260.012114	523508.275988	38.622567
2262.371939	524473.095878	38.627584
2264.348935	525463.857539	38.632602
2266.406700	526447.792060	38.637620
2268.366683	527440.743677	38.642637
2269.976465	528427.795412	38.647655
2272.452823	529423.098866	38.652672
2274.603343	530423.072311	38.657690
2277.150946	531417.022127	38.662708
2279.856983	532401.363739	38.667725
2282.347993	533401.633423	38.672743
2284.406818	534379.203514	38.677760
2286.723147	535384.954136	38.682778
2288.979819	536378.515222	38.687796
2291.152980	537353.148958	38.692813
2293.043082	538357.757251	38.697831
2295.656351	539360.565958	38.702848
2297.490366	540325.694708	38.707866
2299.643748	541293.171061	38.712884
2302.174087	542266.204698	38.717901
2304.049571	543255.227080	38.722919
2306.109996	544221.512999	38.727936
2308.203017	545208.853520	38.732954
2310.110000	546200.631715	38.737972
2312.197647	547187.330765	38.742989
2314.113772	548210.347765	38.748007
2316.676826	549224.583831	38.753024
2318.414492	550253.061242	38.758042
2320.516820	551283.614057	38.763060
2323.015925	552325.537030	38.768077
2325.062989	553360.015088	38.773095
2327.280247	554402.881712	38.778112
2329.554466	555467.774640	38.783130
2331.816339	556533.641221	38.788148
2334.028462	557599.381453	38.793165
2336.404951	558680.587841	38.798183
2338.711573	559749.910285	38.803200
2341.323056	560833.365664	38.808218
2343.885381	561918.398589	38.813236
2346.526397	563002.274575	38.818253
2348.975811	564086.997116	38.823271
2351.582210	565177.530837	38.828288
2353.857251	566282.542439	38.833306
2356.031887	567366.084003	38.838324
2358.581617	568448.519187	38.843341
2360.928185	569564.989492	38.848359
2363.152032	570671.944683	38.853376
2365.748602	571767.497938	38.858394
2367.827531	572866.907765	38.863412
2370.576287	573989.250820	38.868429
2372.371073	575114.311801	38.873447
2375.126738	576214.373913	38.878464
2377.674070	577349.649942	38.883482
2379.588234	578479.860021	38.888500
2382.247839	579600.914800	38.893517
2383.765465	580726.772431	38.898535
2386.675840	581875.823564	38.903552
2388.538614	583033.316569	38.908570
2390.889588	584182.445642	38.913588
2393.348798	585332.953587	38.918605
2395.553203	586507.764012	38.923623
2398.291563	587661.766813	38.928640
2401.165808	588825.312843	38.933658
2403.463708	589976.410267	38.938676
2406.325014	591136.276608	38.943693
2408.711731	592300.469195	38.948711
2411.242819	593453.249181	38.953728
2413.763928	594617.995105	38.958746
2415.929092	595769.658560	38.963764
2419.313965	596917.351511	38.968781
2421.584640	598085.003139	38.973799
2424.201698	599227.788000	38.978816
2426.707368	600369.077120	38.983834
2429.030559	601515.041877	38.988852
2432.017717	602654.074145	38.993869
2434.336384	603803.818995	38.998887
2437.479040	604930.934904	39.003904
2440.892473	606041.276027	39.008922
2443.571975	607154.233119	39.013940
2446.586337	608255.014609	39.018957
2449.119443	609344.608934	39.023975
2452.031818	610428.281353	39.028992
2454.954071	611516.851500	39.034010
2457.035337	612592.597302	39.039028
2459.717090	613645.679715	39.044045
2462.060126	614682.412109	39.049063
2464.902005	615712.363707	39.054080
2467.369871	616726.627957	39.059098
2469.811975	617744.203956	39.064116
2472.293461	618736.528671	39.069133
2474.538601	619769.700685	39.074151
2476.763409	620786.931086	39.079168
2479.175448	621814.233540	39.084186
2481.183099	622835.507866	39.089204
2483.579055	623867.067732	39.094221
2485.985497	624903.874848	39.099239
2487.901812	625941.412782	39.104256
2490.125157	627006.779996	39.109274
2492.222966	628072.711653	39.114292
2494.301408	629144.235095	39.119309
2495.912838	630237.305833	39.124327
2498.088470	631332.119037	39.129344
2500.683577	632454.066365	39.134362
2502.555896	633568.873270	39.139380
2504.998785	634690.408096	39.144397
2507.300096	635836.807638	39.149415
2509.607290	636981.982435	39.154432
2512.373767	638135.839992	39.159450
2514.310383	639306.175144	39.164468
2516.591587	640473.127685	39.169485
2518.681003	641667.920796	39.174503
2521.539252	642850.774531	39.179520
2523.933010	644054.668784	39.184538
2526.414528	645269.080389	39.189556
2528.837699	646473.133292	39.194573
2531.188955	647712.658719	39.199591
2533.323990	648936.162986	39.204608
2536.374904	650179.956909	39.209626
2538.192608	651437.308450	39.214644
2540.930430	652693.652650	39.219661
2543.083833	653964.984727	39.224679
2545.305559	655225.729044	39.229696
2547.917185	656515.692795	39.234714
2550.319958	657815.883755	39.239732
2552.570592	659103.725024	39.244749
2555.081819	660407.340278	39.249767
2558.072864	661709.507344	39.254784
2560.808246	663023.292179	39.259802
2562.495447	664357.979748	39.264820
2565.534424	665661.897964	39.269837
2568.258772	666989.281105	39.274855
2570.673460	668329.817595	39.279872
2573.148289	669666.524159	39.284890
2575.596346	671013.245499	39.289908
2578.497109	672360.795342	39.294925
2580.930537	673702.958532	39.299943
2583.657035	675055.871422	39.304960
2586.202289	676395.593114	39.309978
2588.674305	677749.103685	39.314996
2591.565449	679096.831523	39.320013
2593.789279	680472.502381	39.325031
2596.672827	681829.673916	39.330048
2599.180442	683189.440110	39.335066
2602.044757	684550.833872	39.340084
2605.545744	685899.553212	39.345101
2608.214441	687250.494624	39.350119
2610.658622	688593.278300	39.355136
2613.390715	689951.801044	39.360154
2616.057708	691304.967800	39.365172
2619.142980	692632.848682	39.370189
2621.821663	693971.268675	39.375207
2624.486088	695328.145680	39.380224
2627.730174	696652.326756	39.385242
2629.845316	697954.821033	39.390260
2632.490635	699247.861423	39.395277
2634.921075	700550.515883	39.400295
2637.655355	701838.846898	39.405312
2640.454510	703120.285575	39.410330
2642.755397	704420.353272	39.415348
2645.706559	705708.771142	39.420365
2648.319505	707006.021630	39.425383
2650.475305	708301.716055	39.430400
2653.573789	709598.496726	39.435418
2656.386764	710895.921014	39.440436
2659.673617	712188.118625	39.445453
2661.960293	713479.196088	39.450471
2664.748419	714784.252012	39.455488
2667.412779	716086.999070	39.460506
2669.861280	717405.961534	39.465524
2672.799042	718712.167665	39.470541
2675.518963	720028.348416	39.475559
2677.763182	721350.039578	39.480576
2680.818352	722655.314019	39.485594
2682.878928	723978.843793	39.490612
2686.003711	725310.737983	39.495629
2688.714393	726647.082974	39.500647
2691.158636	727989.284900	39.505664
2693.903882	729328.450345	39.510682
2696.571564	730684.653176	39.515700
2699.227014	732019.093594	39.520717
2701.996794	733378.980383	39.525735
2704.795667	734732.856102	39.530752
2707.545707	736088.142280	39.535770
2709.965347	737447.500337	39.540788
2712.666940	738816.354788	39.545805
2715.480285	740194.629289	39.550823
2718.261297	741577.703695	39.555840
2721.213641	742947.435602	39.560858
2723.821388	744327.789587	39.565876
2726.736147	745698.382769	39.570893
2729.343844	747090.532592	39.575911
2732.099485	748484.826536	39.580928
2734.784498	749869.074596	39.585946
2737.219641	751255.532677	39.590964
2740.288364	752660.165359	39.595981
2742.451764	754061.440904	39.600999
2744.856283	755477.691190	39.606016
2747.639850	756888.693605	39.611034
2750.245811	758321.572707	39.616052
2752.759797	759748.487838	39.621069
2755.374388	761191.853073	39.626087
2757.716757	762623.523049	39.631104
2761.093919	764067.100507	39.636122
2763.930676	765520.033350	39.641140
2766.563685	766962.686038	39.646157
2769.691713	768412.108978	39.651175
2772.291933	769872.841106	39.656192
2775.040313	771324.906254	39.661210
2777.585567	772793.477840	39.666228
2779.973873	774252.399258	39.671245
2782.654922	775736.821725	39.676263
2785.073810	777214.357094	39.681280
2788.025250	778685.712267	39.686298
2790.710821	780186.318809	39.691316
2793.438622	781664.767037	39.696333
2796.121247	783168.585629	39.701351
2798.587819	784670.949101	39.706368
2801.889659	786164.424388	39.711386
2804.015712	787689.708189	39.716404
2806.575334	789196.845970	39.721421
2809.392391	790698.328256	39.726439
2812.235850	792191.254954	39.731456
2814.862601	793678.169410	39.736474
2817.496524	795165.846980	39.741492
2820.056341	796641.369013	39.746509
2823.077942	798135.650997	39.751527
2825.660525	799639.722009	39.756544
2828.620508	801136.504262	39.761562
2831.427462	802645.076237	39.766580
2834.465899	804152.644939	39.771597
2836.644210	805677.928673	39.776615
2839.330945	807205.284152	39.781632
2841.873959	808737.603130	39.786650
2844.656024	810281.172708	39.791668
2847.464584	811833.428822	39.796685
2850.327387	813395.532309	39.801703
2852.646586	814962.053683	39.806720
2855.678866	816543.037327	39.811738
2858.608406	818110.580160	39.816756
2861.180055	819708.567482	39.821773
2864.494644	821307.366965	39.826791
2867.073860	822905.805220	39.831808
2870.505019	824490.839574	39.836826
2873.294729	826099.006980	39.841844
2876.909777	827713.031979	39.846861
2879.841792	829305.471259	39.851879
2882.937014	830904.805030	39.856896
2885.957002	832518.032894	39.861914
2888.646164	834139.291651	39.866932
2891.646079	835736.719192	39.871949
2894.957754	837343.095054	39.876967
2897.745040	838955.093236	39.881984
2900.328300	840575.623442	39.887002
2903.084526	842192.989284	39.892020
2905.912268	843822.333315	39.897037
2909.310267	845451.942267	39.902055
2911.920102	847081.066017	39.907072
2915.056745	848716.192994	39.912090
2917.973386	850350.735540	39.917108
2920.363839	851986.977258	39.922125
2923.762969	853644.473716	39.927143
2926.331144	855302.344119	39.932160
2929.495797	856932.882793	39.937178
2932.465208	858591.260080	39.942196
2935.184415	860255.439684	39.947213
2938.422026	861917.529916	39.952231
2941.403739	863581.536629	39.957248
2944.443973	865233.543716	39.962266
2947.419559	866889.375044	39.967284
2950.542547	868557.806753	39.972301
2953.846088	870211.703032	39.977319
2956.771481	871877.018311	39.982336
2959.620989	873542.366393	39.987354
2962.725744	875208.078084	39.992372
2965.366606	876871.077334	39.997389
2968.200370	878539.670815	40.002407
2971.077148	880209.525789	40.007424
2973.766689	881889.473495	40.012442
2976.673408	883582.142610	40.017460
2979.426792	885266.038554	40.022477
2982.428887	886954.235330	40.027495
2985.104385	888638.036261	40.032512
2988.042892	890334.719914	40.037530
2990.785712	892043.866190	40.042548
2993.248734	893764.800761	40.047565
2996.786603	895480.026375	40.052583
2999.852867	897194.331926	40.057600
3002.696400	898908.735525	40.062618
3005.615682	900619.043144	40.067636
3008.608109	902296.361831	40.072653
3011.584901	903973.760978	40.077671
3014.173551	905643.984328	40.082688
3017.527138	907337.351843	40.087706
3020.489352	909014.780801	40.092724
3023.267743	910700.292859	40.097741
3026.695643	912371.243985	40.102759
3029.444623	914066.117847	40.107776
3032.764552	915757.204597	40.112794
3035.744744	917448.690116	40.117812
3038.528250	919151.783529	40.122829
3041.672289	920854.476945	40.127847
3044.501980	922575.976840	40.132864
3047.914033	924282.347010	40.137882
3050.838434	925995.258420	40.142900
3053.872525	927713.837525	40.147917
3057.018595	929445.360443	40.152935
3059.838017	931188.256027	40.157952
3062.700716	932905.383695	40.162970
3065.682131	934673.065082	40.167988
3068.413663	936428.806295	40.173005
3071.712010	938191.810630	40.178023
3074.494160	939958.612189	40.183040
3077.590421	941732.701708	40.188058
3080.587881	943515.762449	40.193076
3083.895050	945300.453602	40.198093
3087.739689	947068.680306	40.203111
3090.567005	948865.305871	40.208128
3093.975338	950659.203661	40.213146
3096.954963	952442.334292	40.218164
3100.202158	954226.896982	40.223181
3103.248677	956049.180212	40.228199
3106.175038	957904.956978	40.233216
3109.489371	959753.521977	40.238234
3112.547969	961589.806776	40.243252
3116.170012	963451.113150	40.248269
3119.917743	965280.635376	40.253287
3122.963387	967139.280633	40.258304
3126.400633	968975.197612	40.263322
3129.853433	970813.745601	40.268340
3132.475364	972665.890021	40.273357
3135.664110	974518.513104	40.278375
3138.327188	976375.595962	40.283392
3141.589470	978220.574121	40.288410
3144.530135	980086.932633	40.293428
3147.117172	981964.233192	40.298445
3150.475116	983834.265686	40.303463
3152.989764	985703.337290	40.308480
3156.091003	987593.495810	40.313498
3159.144988	989500.057460	40.318516
3161.790598	991408.672934	40.323533
3165.127764	993321.977264	40.328551
3167.887986	995242.408810	40.333568
3170.862961	997160.503601	40.338586
3173.991473	999096.763227	40.343604
3176.861829	1001044.732013	40.348621
3180.432768	1002996.863970	40.353639
3183.460702	1004943.366847	40.358656
3186.800828	1006901.754249	40.363674
3190.143869	1008841.236590	40.368692
3193.017241	1010812.690112	40.373709
3196.481996	1012757.878482	40.378727
3199.348205	1014724.185325	40.383744
3202.346624	1016691.525309	40.388762
3205.724099	1018655.791353	40.393780
3208.275230	1020634.597223	40.398797
3211.426458	1022610.478500	40.403815
3214.013097	1024590.106036	40.408832
3217.517072	1026552.164321	40.413850
3220.501326	1028491.980809	40.418868
3223.627377	1030447.323963	40.423885
3226.738938	1032397.736968	40.428903
3229.508230	1034366.341872	40.433920
3232.706223	1036323.183379	40.438938
3236.042582	1038278.639104	40.443956
3239.134454	1040269.886212	40.448973
3242.558044	1042255.354086	40.453991
3245.215171	1044251.604862	40.459008
3248.243472	1046245.150050	40.464026
3251.614279	1048254.381936	40.469044
3254.397164	1050284.246929	40.474061
3257.693360	1052306.837611	40.479079
3260.911949	1054350.431319	40.484096
3264.000287	1056399.345221	40.489114
3267.242506	1058433.828722	40.494132
3270.075055	1060504.126004	40.499149
3273.624744	1062577.654776	40.504167
3276.747244	1064661.412826	40.509184
3280.259023	1066747.769925	40.514202
3283.530830	1068822.919987	40.519220
3286.514455	1070939.032846	40.524237
3290.121136	1073032.951750	40.529255
3293.380589	1075151.414949	40.534272
3296.795950	1077261.562509	40.539290
3299.955226	1079374.765261	40.544308
3303.237156	1081512.770910	40.549325
3306.500229	1083632.916567	40.554343
3310.198327	1085773.484337	40.559360
3313.568996	1087910.491856	40.564378
3316.915386	1090037.205265	40.569396
3320.031895	1092190.433367	40.574413
3323.435322	1094343.808868	40.579431
3326.823977	1096503.772782	40.584448
3330.035621	1098647.929223	40.589466
3333.374049	1100811.330466	40.594484
3336.674488	1102976.729936	40.599501
3339.963776	1105149.740010	40.604519
3343.336793	1107330.334588	40.609536
3346.290213	1109484.890628	40.614554
3350.033238	1111672.325297	40.619572
3353.597408	1113858.137445	40.624589
3357.507313	1116039.864652	40.629607
3360.973039	1118208.327667	40.634624
3364.152111	1120391.443079	40.639642
3367.459768	1122564.720438	40.644660
3371.142860	1124759.356561	40.649677
3374.448211	1126932.564289	40.654695
3377.911735	1129120.887272	40.659712
3381.136940	1131307.307334	40.664730
3384.210630	1133488.399938	40.669748
3387.124326	1135698.839033	40.674765
3390.657079	1137903.900356	40.679783
3393.827315	1140105.454316	40.684800
3396.968688	1142311.773919	40.689818
3400.398483	1144526.960276	40.694836
3403.382157	1146749.514910	40.699853
3406.451044	1148973.859756	40.704871
3409.845419	1151212.890038	40.709888
3413.245925	1153457.481218	40.714906
3416.994207	1155694.452275	40.719924
3420.135256	1157947.077296	40.724941
3423.137500	1160183.202399	40.729959
3426.093050	1162451.742652	40.734976
3429.078229	1164722.498391	40.739994
3432.596746	1166976.174010	40.745012
3435.727259	1169253.973068	40.750016
3439.466427	1171452.374022	40.755021
3442.721581	1173612.970646	40.760026
3445.974230	1175696.430959	40.765031
3449.627989	1177687.330233	40.770036
3452.747316	1179623.878340	40.775040
3455.474640	1181478.247404	40.780045
3459.080869	1183238.175903	40.785050
3461.906471	1184939.968613	40.790055
3464.547814	1186557.721964	40.795060
3467.221101	1188092.512739	40.800064
3469.726583	1189540.217616	40.805069
3472.587742	1190923.656622	40.810074
3474.823553	1192229.702944	40.815079
3477.441451	1193455.995118	40.820084
3479.898997	1194617.890464	40.825088
3482.194807	1195690.648832	40.830093
3483.746463	1196712.528668	40.835098
3485.610910	1197671.655895	40.840103
3487.566572	1198552.808356	40.845108
3489.253862	1199402.990555	40.850112
3490.883875	1200174.159616	40.855117
3492.388869	1200898.623620	40.860122
3493.968017	1201576.181933	40.865127
3495.414636	1202185.041202	40.870132
3496.671477	1202776.609776	40.875136
3497.880557	1203295.001988	40.880141
3499.037525	1203780.826086	40.885146
3500.312252	1204226.284400	40.890151
3501.968266	1204618.411377	40.895156
3502.183397	1204977.854092	40.900160
3503.457427	1205327.914432	40.905165
3504.062066	1205623.529954	40.910170
3504.833118	1205889.775584	40.915175
3506.170064	1206130.150222	40.920180
3506.468550	1206337.145988	40.925184
3507.522078	1206516.279754	40.930189
3508.470684	1206669.569609	40.935194
3508.762714	1206791.488216	40.940199
3509.444866	1206891.513811	40.945204
3509.931567	1206976.582163	40.950208
3510.729368	1207035.838468	40.955213
3511.355680	1207083.413603	40.960218
3511.768323	1207105.358106	40.965223
3512.398798	1207091.672260	40.970228
3512.621353	1207077.772548	40.975232
3513.520643	1207035.941208	40.980237
3513.596608	1206982.442496	40.985242
3513.962101	1206911.285042	40.990247
3514.740288	1206829.192401	40.995252
3514.718136	1206749.665832	41.000256
3514.770651	1206639.118404	41.005261
3515.312027	1206515.091819	41.010266
3515.328072	1206392.085579	41.015271
3515.413445	1206240.584718	41.020276
3515.649643	1206103.950921	41.025280
3516.323229	1205949.065502	41.030285
3516.749701	1205792.717012	41.035290
3516.761238	1205602.607604	41.040295
3517.386557	1205411.265659	41.045300
3517.315363	1205224.810188	41.050304
3517.657875	1205018.038995	41.055309
3517.685596	1204808.968526	41.060314
3517.765716	1204592.477394	41.065319
3517.927908	1204351.409078	41.070324
3518.318490	1204118.258375	41.075328
3518.259090	1203875.985805	41.080333
3518.682681	1203633.059855	41.085338
3518.590998	1203390.957170	41.090343
3519.142211	1203137.206935	41.095348
3518.865601	1202868.768511	41.100352
3519.302210	1202595.323492	41.105357
3519.332456	1202329.431385	41.110362
3519.030511	1202064.049026	41.115367
3519.624123	1201779.752143	41.120372
3519.402023	1201489.572465	41.125376
3519.466449	1201212.458018	41.130381
3519.850309	1200922.427844	41.135386
3519.673991	1200631.254323	41.140391
3519.653661	1200334.692407	41.145396
3519.694978	1200050.390824	41.150400
3520.062924	1199738.347616	41.155405
3519.958010	1199443.342882	41.160410
3520.145301	1199120.410036	41.165415
3520.215408	1198800.666135	41.170420
3520.156716	1198502.691380	41.175424
3520.432726	1198194.510379	41.180429
3520.532872	1197856.405548	41.185434
3520.358903	1197537.467894	41.190439
3520.507257	1197212.357139	41.195444
3520.239102	1196895.459918	41.200448
3520.300969	1196565.629777	41.205453
3520.700541	1196234.127143	41.210458
3520.554613	1195906.072481	41.215463
3520.526412	1195567.462982	41.220468
3520.523804	1195247.979768	41.225472
3520.793479	1194914.066457	41.230477
3520.879697	1194577.438688	41.235482
3520.420737	1194241.160438	41.240487
3520.625681	1193905.220458	41.245492
3520.557308	1193568.270529	41.250496
3520.554807	1193212.315337	41.255501
3520.899936	1192875.627758	41.260506
3520.624207	1192534.229766	41.265511
3520.748940	1192186.355204	41.270516
3520.249713	1191839.781280	41.275520
3520.545288	1191506.206758	41.280525
3520.817196	1191161.057486	41.285530
3520.486663	1190812.413637	41.290535
3520.494051	1190469.610886	41.295540
3520.131960	1190122.335238	41.300544
3520.265909	1189771.947010	41.305549
3520.244534	1189428.891970	41.310554
3520.161698	1189102.085915	41.315559
3520.383872	1188754.434111	41.320564
3520.067383	1188408.727854	41.325568
3520.044933	1188056.180851	41.330573
3520.253858	1187724.350787	41.335578
3520.033191	1187387.210544	41.340583
3520.235993	1187043.396130	41.345588
3520.105611	1186691.150015	41.350592
3520.449935	1186347.172004	41.355597
3520.122450	1186001.776918	41.360602
3519.916834	1185661.135787	41.365607
3520.177436	1185314.469270	41.370612
3520.233615	1184965.461399	41.375616
3520.027389	1184612.333741	41.380621
3520.094619	1184268.827795	41.385626
3520.142129	1183923.796856	41.390631
3519.754040	1183573.733389	41.395636
3519.934443	1183226.563990	41.400640
3519.844795	1182881.956812	41.405645
3519.738960	1182532.435310	41.410650
3519.636779	1182190.137146	41.415655
3519.976731	1181846.237503	41.420660
3519.938303	1181504.824917	41.425664
3519.862720	1181156.900189	41.430669
3519.868379	1180807.244083	41.435674
3519.822514	1180463.033880	41.440679
3519.918506	1180097.214611	41.445684
3520.041024	1179759.897991	41.450688
3520.143470	1179405.234822	41.455693
3520.046506	1179046.530528	41.460698
3519.631326	1178706.126079	41.465703
3520.025646	1178333.822988	41.470708
3519.867927	1177982.779097	41.475712
3519.605067	1177626.830101	41.480717
3519.869040	1177298.279932	41.485722
3520.088330	1176946.821361	41.490727
3519.861516	1176584.670885	41.495732
3519.464594	1176231.004029	41.500736
3519.548109	1175875.914670	41.505741
3519.791572	1175531.989782	41.510746
3519.466501	1175190.492059	41.515751
3519.398253	1174828.193191	41.520756
3519.442975	1174477.256348	41.525760
3519.411097	1174141.957168	41.530765
3519.369890	1173790.045474	41.535770
3519.285579	1173432.460187	41.540775
3519.622722	1173095.430072	41.545780
3519.594448	1172755.326638	41.550784
3519.596649	1172396.524480	41.555789
3519.649029	1172046.742843	41.560794
3519.154120	1171701.554912	41.565799
3519.720173	1171343.813514	41.570804
3519.325374	1170990.544837	41.575808
3519.142551	1170653.348153	41.580813
3519.090098	1170309.976203	41.585818
3519.073766	1169958.650749	41.590823
3519.106645	1169607.670944	41.595828
3518.659770	1169279.014870	41.600832
3518.446414	1168933.786081	41.605837
3518.903523	1168590.311433	41.610842
3518.926368	1168255.190781	41.615847
3518.773484	1167904.693338	41.620852
3518.903455	1167563.942162	41.625856
3518.792030	1167236.329303	41.630861
3518.732094	1166890.562608	41.635866
3518.483582	1166541.688680	41.640871
3518.690389	1166199.986259	41.645876
3518.364303	1165869.868366	41.650880
3518.516296	1165533.041161	41.655885
3518.511536	1165198.862145	41.660890
3518.175098	1164859.900126	41.665895
3518.790142	1164516.887272	41.670900
3518.645638	1164183.138610	41.675904
3518.356848	1163838.057795	41.680909
3518.582111	1163506.660937	41.685914
3518.309571	1163170.979592	41.690919
3518.508654	1162825.279329	41.695924
3517.956274	1162493.285091	41.700928
3518.111084	1162170.507397	41.705933
3518.274078	1161835.330103	41.710938
3518.064598	1161507.469019	41.715943
3517.937944	1161167.288335	41.720948
3517.994367	1160838.869111	41.725952
3517.970221	1160492.201087	41.730957
3518.212923	1160173.633655	41.735962
3518.008206	1159845.100672	41.740967
3518.405989	1159496.973989	41.745972
3518.229933	1159159.034478	41.750976
3518.040651	1158830.340854	41.755981
3518.305521	1158493.231299	41.760986
3517.783490	1158165.969135	41.765991
3517.701052	1157814.405847	41.770996
3517.752282	1157509.230799	41.776000
3517.621333	1157168.696877	41.781005
3517.860528	1156830.255290	41.786010
3517.490333	1156512.701527	41.791015
3517.597596	1156183.793338	41.796020
3517.318953	1155856.725503	41.801024
3517.466309	1155535.432660	41.806029
3517.585305	1155206.082929	41.811034
3517.261834	1154885.774029	41.816039
3517.129774	1154559.358245	41.821044
3517.199170	1154239.418376	41.826048
3517.279264	1153917.659235	41.831053
3517.182829	1153592.218532	41.836058
3517.065940	1153276.509572	41.841063
3517.358028	1152954.088717	41.846068
3516.794309	1152639.645602	41.851072
3517.052930	1152313.310067	41.856077
3517.068323	1151996.366569	41.861082
3516.869782	1151678.776506	41.866087
3517.146549	1151355.692239	41.871092
3517.079458	1151041.071834	41.876096
3516.929533	1150719.817872	41.881101
3517.069607	1150408.250376	41.886106
3516.693745	1150092.108993	41.891111
3516.945215	1149762.870234	41.896116
3516.814764	1149456.594721	41.901120
3516.670008	1149130.128415	41.906125
3516.819376	1148820.833558	41.911130
3516.681621	1148504.368270	41.916135
3516.688314	1148194.397055	41.921140
3516.846338	1147883.435278	41.926144
3516.664740	1147559.151607	41.931149
3516.186027	1147255.269045	41.936154
3516.247821	1146948.816218	41.941159
3516.282510	1146629.462032	41.946164
3516.438380	1146327.980218	41.951168
3516.707600	1146023.524471	41.956173
3516.398962	1145704.644774	41.961178
3516.180925	1145388.479729	41.966183
3516.374635	1145085.593740	41.971188
3516.077993	1144784.193120	41.976192
3516.327901	1144476.617857	41.981197
3516.197299	1144165.674233	41.986202
3516.101374	1143871.204359	41.991207
3516.395456	1143556.552007	41.996212
3516.463994	1143249.693793	42.001216
3515.780166	1142930.518783	42.006221
3516.074610	1142630.035938	42.011226
3515.724357	1142336.281155	42.016231
3515.775717	1142024.707430	42.021236
3515.928973	1141730.456691	42.026240
3515.785704	1141420.397086	42.031245
3515.760497	1141123.770546	42.036250
3515.419739	1140830.025426	42.041255
3515.517228	1140522.150405	42.046260
3515.412008	1140233.266855	42.051264
3515.284032	1139929.474337	42.056269
3515.949026	1139640.241824	42.061274
3515.529249	1139352.405827	42.066279
3515.694510	1139051.741125	42.071284
3515.186875	1138756.390032	42.076288
3515.107608	1138451.081115	42.081293
3515.355348	1138170.663903	42.086298
3515.234101	1137889.058649	42.091303
3515.589509	1137595.304220	42.096308
3515.489290	1137295.248098	42.101312
3515.074088	1137003.106699	42.106317
3515.358069	1136700.485273	42.111322
3515.137137	1136415.874967	42.116327
3515.367907	1136116.362278	42.121332
3515.384608	1135830.162162	42.126336
3515.504232	1135544.024624	42.131341
3515.446245	1135247.359366	42.136346
3515.198228	1134959.636404	42.141351
3515.080275	1134666.177663	42.146356
3514.840170	1134381.841339	42.151360
3515.370159	1134079.979837	42.156365
3514.987574	1133788.795952	42.161370
3514.652964	1133511.268225	42.166375
3514.646894	1133231.771786	42.171380
3514.760107	1132948.155567	42.176384
3514.929713	1132655.298446	42.181389
3514.962380	1132372.709960	42.186394
3514.895649	1132088.317339	42.191399
3514.939561	1131794.578279	42.196404
3515.040852	1131514.308637	42.201408
3514.809246	1131230.182381	42.206413
3514.628391	1130945.367265	42.211418
3514.425512	1130672.992191	42.216423
3514.726505	1130378.277116	42.221428
3514.184716	1130105.928827	42.226432
3514.175920	1129816.176810	42.231437
3514.317594	1129543.401967	42.236442
3514.026269	1129277.815145	42.241447
3513.987296	1128994.868840	42.246452
3513.795874	1128727.051229	42.251456
3513.901543	1128458.790855	42.256461
3514.038073	1128181.382751	42.261466
3514.141720	1127926.979825	42.266471
3514.225506	1127641.183493	42.271476
3514.138575	1127390.019884	42.276480
3514.078649	1127121.814576	42.281485
3514.067294	1126838.558952	42.286490
3514.134301	1126564.121922	42.291495
3513.941345	1126292.091807	42.296500
3513.609144	1126021.402616	42.301504
3513.507288	1125764.076275	42.306509
3513.655148	1125477.677696	42.311514
3513.468719	1125217.674903	42.316519
3513.592073	1124960.558150	42.321524
3513.705404	1124696.389013	42.326528
3513.424150	1124425.039457	42.331533
3513.442738	1124160.193245	42.336538
3513.398662	1123908.858581	42.341543
3513.564892	1123633.873753	42.346548
3513.395108	1123384.628992	42.351552
3513.360402	1123120.406238	42.356557
3513.524231	1122859.850130	42.361562
3513.092137	1122607.090236	42.366567
3513.167222	1122344.619717	42.371572
3513.055488	1122090.164206	42.376576
3512.862292	1121837.804576	42.381581
3513.162963	1121592.302225	42.386586
3512.764503	1121343.856795	42.391591
3512.810774	1121080.567191	42.396596
3513.152166	1120825.691174	42.401600
3512.856744	1120583.668828	42.406605
3513.009695	1120326.514516	42.411610
3512.473785	1120076.699521	42.416615
3512.900575	1119821.285372	42.421620
3512.547574	1119587.037421	42.426624
3512.807632	1119334.389696	42.431629
3512.720313	1119085.788068	42.436634
3512.454531	1118845.301531	42.441639
3512.608260	1118591.874169	42.446644
3512.436369	1118351.064157	42.451648
3512.523936	1118102.388040	42.456653
3512.817621	1117857.001201	42.461658
3512.571579	1117621.601501	42.466663
3512.418319	1117368.262057	42.471668
3512.400268	1117121.654120	42.476672
3512.558237	1116887.966182	42.481677
3512.566204	1116643.142564	42.486682
3512.246984	1116391.404356	42.491687
3512.508152	1116146.230412	42.496692
3512.400570	1115912.638979	42.501696
3512.227637	1115670.469494	42.506701
3512.305049	1115440.449100	42.511706
3512.133486	1115191.299206	42.516711
3512.509183	1114953.773317	42.521716
3512.522025	1114717.917368	42.526720
3512.516531	1114469.945957	42.531725
3512.231857	1114218.195301	42.536730
3512.205966	1113986.413349	42.541735
3512.261585	1113742.974968	42.546740
3512.206861	1113505.169762	42.551744
3512.277975	1113261.802355	42.556749
3512.410186	1113022.991382	42.561754
3511.947015	1112793.804782	42.566759
3511.989152	1112544.305967	42.571764
3512.196613	1112320.329623	42.576768
3511.931906	1112081.828279	42.581773
3511.863686	1111846.813264	42.586778
3511.613582	1111617.255163	42.591783
3511.967848	1111375.568012	42.596788
3511.754633	1111155.523541	42.601792
3511.847593	1110914.049460	42.606797
3511.689258	1110679.856841	42.611802
3511.429995	1110459.600627	42.616807
3511.377366	1110226.802009	42.621812
3511.668169	1110001.474843	42.626816
3511.487482	1109773.353198	42.631821
3511.733298	1109550.781817	42.636826
3511.603578	1109321.964632	42.641831
3511.255261	1109090.787831	42.646836
3511.271320	1108868.703230	42.651840
3511.469483	1108644.097946	42.656845
3511.352065	1108417.244531	42.661850
3511.541854	1108201.403264	42.666855
3511.839099	1107971.217415	42.671860
3511.924799	1107741.724776	42.676864
3511.515673	1107513.735791	42.681869
3511.807848	1107281.421084	42.686874
3511.356474	1107050.078054	42.691879
3511.610453	1106822.332444	42.696884
3511.244406	1106611.483661	42.701888
3511.224431	1106377.940142	42.706893
3511.379483	1106151.614701	42.711898
3511.173443	1105940.331324	42.716903
3511.151451	1105721.942727	42.721908
3511.371643	1105500.258430	42.726912
3511.032009	1105262.803740	42.731917
3510.978718	1105045.729920	42.736922
3510.860717	1104842.984595	42.741927
3511.191029	1104620.577391	42.746932
3510.815043	1104410.408151	42.751936
3510.629772	1104190.551585	42.756941
3511.336249	1103978.658874	42.761946
3510.729888	1103769.266771	42.766951
3510.642169	1103547.457314	42.771956
3510.847641	1103343.169282	42.776960
3510.919400	1103126.952941	42.781965
3511.110263	1102918.638518	42.786970
3510.783539	1102699.890981	42.791975
3511.340402	1102464.840682	42.796980
3510.995944	1102247.128778	42.801985
3510.830410	1102043.808200	42.806989
3510.747122	1101819.537934	42.811994
3510.639694	1101620.396642	42.816999
3510.714020	1101402.581675	42.822004
3510.557312	1101200.279138	42.827009
3510.776908	1100976.879716	42.832013
3510.537458	1100767.501737	42.837018
3510.752424	1100557.658449	42.842023
3510.882136	1100339.313526	42.847028
3511.004285	1100130.138044	42.852033
3510.490249	1099919.529678	42.857037
3510.578515	1099702.504200	42.862042
3510.230216	1099501.412365	42.867047
3510.524647	1099291.506793	42.872052
3510.416660	1099088.639053	42.877057
3510.344720	1098884.132286	42.882061
3510.639451	1098665.596909	42.887066
3510.186949	1098464.770500	42.892071
3510.546308	1098243.147450	42.897076
3510.490440	1098055.819578	42.902081
3510.317289	1097847.369387	42.907085
3510.292465	1097636.878329	42.912090
3510.061336	1097441.715714	42.917095
3510.027825	1097241.444320	42.922100
3510.213104	1097034.721017	42.927105
3510.226856	1096829.548501	42.932109
3510.429336	1096639.929016	42.937114
3510.039753	1096435.668888	42.942119
3509.936061	1096230.875643	42.947124
3509.585951	1096037.116868	42.952129
3509.721754	1095837.339593	42.957133
3509.820316	1095643.301479	42.962138
3509.854816	1095446.588011	42.967143
3509.854306	1095247.002751	42.972148
3509.907943	1095051.706985	42.977153
3509.768897	1094872.032900	42.982157
3509.868523	1094666.572842	42.987162
3509.554921	1094477.345341	42.992167
3509.664239	1094277.801954	42.997172
3509.544521	1094093.696769	43.002177
3509.513168	1093902.584379	43.007181
3509.494291	1093708.591967	43.012186
3509.601875	1093524.429994	43.017191
3509.409292	1093331.696933	43.022196
3509.700738	1093152.469169	43.027201
3509.741233	1092956.812865	43.032205
3509.657741	1092751.501761	43.037210
3509.292351	1092568.150979	43.042215
3509.619681	1092388.509134	43.047220
3509.460800	1092187.879901	43.052225
3509.286758	1092006.297545	43.057229
3509.365425	1091816.242290	43.062234
3509.347726	1091642.377002	43.067239
3509.186578	1091445.837666	43.072244
3509.454495	1091265.306670	43.077249
3509.724405	1091074.236408	43.082253
3509.499056	1090884.390075	43.087258
3509.498509	1090707.427751	43.092263
3509.300066	1090519.000602	43.097268
3509.194668	1090329.881212	43.102273
3509.148017	1090148.215646	43.107277
3509.274914	1089949.180371	43.112282
3508.957178	1089774.729983	43.117287
3509.390307	1089590.763867	43.122292
3509.555513	1089406.931430	43.127297
3509.217107	1089228.156618	43.132301
3509.264298	1089032.166016	43.137306
3509.023873	1088864.187341	43.142311
3509.320987	1088670.154163	43.147316
3509.500532	1088479.965410	43.152321
3509.142731	1088294.936064	43.157325
3509.311439	1088113.645946	43.162330
3509.120276	1087932.504859	43.167335
3509.528558	1087743.019107	43.172340
3509.196336	1087569.266717	43.177345
3508.709101	1087388.731150	43.182349
3508.662882	1087205.433921	43.187354
3508.861134	1087040.201235	43.192359
3509.052721	1086847.461890	43.197364
3509.037482	1086680.336856	43.202369
3508.802890	1086503.851022	43.207373
3508.833714	1086328.082445	43.212378
3508.595964	1086160.307202	43.217383
3508.848848	1085979.986282	43.222388
3508.699868	1085807.201636	43.227393
3508.400176	1085641.720914	43.232397
3508.782569	1085452.542983	43.237402
3508.762643	1085288.922509	43.242407
3508.377728	1085110.978366	43.247412
3508.519749	1084951.155425	43.252417
3508.358709	1084779.969776	43.257421
3508.842214	1084604.358519	43.262426
3508.460965	1084429.363379	43.267431
3508.344086	1084260.263268	43.272436
3508.303875	1084105.143323	43.277441
3508.293946	1083929.975083	43.282445
3508.515043	1083772.309733	43.287450
3508.198182	1083608.975283	43.292455
3508.014186	1083442.162057	43.297460
3508.560386	1083278.483766	43.302465
3508.285163	1083113.209749	43.307469
3508.336083	1082943.945205	43.312474
3508.040904	1082775.883206	43.317479
3508.370847	1082606.658123	43.322484
3508.159888	1082450.943737	43.327489
3508.154041	1082280.708866	43.332493
3508.499308	1082126.524047	43.337498
3508.110939	1081963.631557	43.342503
3508.480140	1081793.127851	43.347508
3508.082911	1081634.831029	43.352513
3507.960241	1081466.987978	43.357517
3508.193789	1081294.380695	43.362522
3507.856630	1081147.091330	43.367527
3508.091501	1080987.520442	43.372532
3507.905651	1080833.002774	43.377537
3507.950217	1080670.096226	43.382541
3508.209626	1080502.448350	43.387546
3508.070210	1080352.130776	43.392551
3508.026936	1080194.789184	43.397556
3508.092787	1080044.429317	43.402561
3508.005640	1079878.354506	43.407565
3508.210363	1079707.236940	43.412570
3508.169211	1079559.759964	43.417575
3508.172910	1079390.104912	43.422580
3507.919277	1079232.674243	43.427585
3507.568137	1079072.568053	43.432589
3507.905240	1078896.413040	43.437594
3508.080060	1078763.082288	43.442599
3507.888280	1078594.010496	43.447604
3507.905545	1078432.577182	43.452609
3507.781173	1078270.586541	43.457613
3507.897055	1078117.669849	43.462618
3507.417913	1077970.030061	43.467623
3507.589589	1077809.416744	43.472628
3508.081332	1077662.184650	43.477633
3507.819021	1077502.209716	43.482637
3507.839294	1077353.223073	43.487642
3507.576936	1077201.494960	43.492647
3507.359860	1077052.443201	43.497652
3507.431278	1076900.843760	43.502657
3507.496907	1076747.224930	43.507661
3507.805306	1076597.882204	43.512666
3507.649600	1076459.173108	43.517671
3507.626754	1076313.717627	43.522676
3507.480354	1076146.194762	43.527681
3507.137168	1076001.839921	43.532685
3507.782638	1075854.821857	43.537690
3507.489987	1075710.739066	43.542695
3507.730164	1075549.663909	43.547700
3507.695653	1075403.898042	43.552705
3507.691952	1075251.016797	43.557709
3507.619885	1075097.086145	43.562714
3507.595657	1074940.646287	43.567719
3507.888161	1074785.302275	43.572724
3507.555666	1074642.734533	43.577729
3507.773836	1074497.671226	43.582733
3507.235279	1074341.971263	43.587738
3507.463168	1074198.531247	43.592743
3507.339970	1074046.212291	43.597748
3507.220903	1073895.809541	43.602753
3507.122356	1073746.359865	43.607757
3507.484292	1073609.414340	43.612762
3506.847289	1073476.664599	43.617767
3506.724490	1073330.281588	43.622772
3507.166874	1073193.408467	43.627777
3506.708175	1073052.741411	43.632781
3506.889871	1072907.353716	43.637786
3507.009739	1072777.824932	43.642791
3506.686893	1072634.050292	43.647796
3506.881679	1072518.530500	43.652801
3506.666839	1072370.023175	43.657805
3506.757886	1072225.304874	43.662810
3506.804576	1072102.017724	43.667815
3506.690082	1071958.094915	43.672820
3506.926693	1071835.443114	43.677825
3506.489441	1071698.581401	43.682829
3506.645231	1071569.882968	43.687834
3506.733934	1071432.639686	43.692839
3506.606356	1071300.041490	43.697844
3506.697664	1071157.216952	43.702849
3506.550464	1071030.477836	43.707853
3506.674491	1070909.361546	43.712858
3506.355772	1070776.013266	43.717863
3506.294340	1070651.750149	43.722868
3506.610075	1070521.366804	43.727873
3506.504518	1070400.853777	43.732877
3506.739393	1070258.270505	43.737882
3506.607492	1070126.990298	43.742887
3506.836497	1069993.628878	43.747892
3506.841463	1069869.144823	43.752897
3506.481703	1069731.932786	43.757901
3506.662937	1069589.533209	43.762906
3506.612355	1069471.393981	43.767911
3506.604440	1069336.998127	43.772916
3506.492627	1069205.692533	43.777921
3506.444409	1069071.873649	43.782925
3506.264463	1068945.380096	43.787930
3505.984707	1068827.553162	43.792935
3506.540620	1068687.375930	43.797940
3506.353216	1068574.143437	43.802945
3506.083595	1068440.634055	43.807949
3506.394247	1068311.737422	43.812954
3506.180975	1068193.885915	43.817959
3506.281237	1068066.268201	43.822964
3506.461625	1067957.193375	43.827969
3505.919985	1067834.964838	43.832973
3505.794790	1067700.067350	43.837978
3505.808539	1067587.454501	43.842983
3506.051776	1067471.435620	43.847988
3506.326640	1067354.255022	43.852993
3505.986718	1067238.327259	43.857997
3506.297248	1067110.267979	43.863002
3505.959780	1067000.105308	43.868007
3506.356123	1066873.469032	43.873012
3506.116987	1066751.647414	43.878017
3506.346168	1066640.903292	43.883021
3506.517080	1066512.179768	43.888026
3506.222927	1066384.780269	43.893031
3505.935075	1066253.721532	43.898036
3506.042410	1066143.179818	43.903041
3505.310187	1066037.680070	43.908045
3505.841940	1065916.771085	43.913050
3506.203305	1065806.180747	43.918055
3506.008862	1065685.963479	43.923060
3506.050901	1065564.165384	43.928065
3505.789186	1065450.399611	43.933069
3506.003966	1065322.891635	43.938074
3505.903881	1065210.441165	43.943079
3505.919846	1065102.972241	43.948084
3505.649430	1064985.061191	43.953089
3505.952406	1064879.561093	43.958093
3506.375790	1064767.207761	43.963098
3506.111693	1064636.780013	43.968103
3505.946510	1064502.965132	43.973108
3506.049922	1064387.577656	43.978113
3506.198027	1064263.327659	43.983117
3506.211490	1064158.342526	43.988122
3505.974098	1064034.535757	43.993127
3505.935053	1063907.421650	43.998132
3505.930152	1063797.236126	44.003137
3505.809585	1063686.393794	44.008141
3506.039976	1063569.235980	44.013146
3505.876656	1063454.835224	44.018151
3505.654968	1063331.106252	44.023156
3506.028843	1063224.119073	44.028161
3505.644293	1063115.329816	44.033165
3506.007181	1062999.485475	44.038170
3505.733191	1062883.069843	44.043175
3506.043946	1062759.240303	44.048180
3505.824599	1062645.698196	44.053185
3505.494150	1062542.567658	44.058189
3505.722097	1062420.284213	44.063194
3505.515450	1062307.118051	44.068199
3505.496688	1062208.454113	44.073204
3506.010262	1062084.672244	44.078209
3505.552379	1061969.615240	44.083213
3505.758884	1061857.912035	44.088218
3505.181162	1061760.294793	44.093223
3505.786250	1061636.487770	44.098228
3505.577835	1061543.330607	44.103233
3505.440935	1061432.060407	44.108237
3505.656626	1061320.826160	44.113242
3505.401065	1061210.822629	44.118247
3505.601575	1061098.719883	44.123252
3505.880208	1060994.786023	44.128257
3505.290600	1060882.809012	44.133261
3505.605404	1060778.672544	44.138266
3505.523832	1060679.702668	44.143271
3505.456329	1060563.011317	44.148276
3505.497878	1060449.477175	44.153281
3505.267080	1060346.096431	44.158285
3505.697916	1060238.464049	44.163290
3505.763944	1060140.808315	44.168295
3505.627604	1060022.479781	44.173300
3505.540874	1059922.823045	44.178305
3505.287700	1059806.916653	44.183309
3505.760540	1059685.013605	44.188314
3505.440664	1059585.485466	44.193319
3505.589088	1059479.714611	44.198324
3505.302949	1059378.443605	44.203329
3505.372757	1059281.927746	44.208333
3505.629267	1059169.005981	44.213338
3505.396000	1059051.057786	44.218343
3505.467349	1058953.187478	44.223348
3505.362529	1058853.803324	44.228353
3505.075939	1058743.081320	44.233357
3505.407336	1058625.897915	44.238362
3505.426206	1058530.051539	44.243367
3505.416535	1058426.116682	44.248372
3505.429908	1058319.960490	44.253377
3505.393518	1058214.003111	44.258381
3505.414140	1058100.134978	44.263386
3504.921015	1057995.982629	44.268391
3505.319479	1057900.448121	44.273396
3505.409091	1057796.485034	44.278401
3505.135500	1057699.419973	44.283405
3505.185012	1057584.283996	44.288410
3504.982935	1057498.861035	44.293415
3504.983367	1057395.964862	44.298420
3505.469708	1057304.933808	44.303425
3504.895043	1057208.584116	44.308429
3505.389377	1057101.843498	44.313434
3505.196875	1057008.125178	44.318439
3505.492447	1056888.983703	44.323444
3505.358094	1056792.168789	44.328449
3505.356583	1056697.450168	44.333453
3505.252333	1056590.990969	44.338458
3504.817563	1056488.342252	44.343463
3504.780113	1056394.780687	44.348468
3505.100047	1056291.040363	44.353473
3504.846358	1056192.596368	44.358477
3505.025601	1056092.441047	44.363482
3505.069372	1055995.486435	44.368487
3504.916607	1055901.068156	44.373492
3505.074517	1055797.923476	44.378497
3504.563167	1055713.873012	44.383501
3504.843280	1055612.921372	44.388506
3504.522280	1055530.475165	44.393511
3504.441235	1055435.940729	44.398516
3504.517603	1055346.486967	44.403521
3504.745600	1055258.452526	44.408525
3504.883180	1055163.877422	44.413530
3504.569503	1055061.182179	44.418535
3504.652494	1054976.733425	44.423540
3504.968553	1054885.401342	44.428545
3504.359770	1054799.232406	44.433549
3504.540214	1054704.449586	44.438554
3504.291321	1054621.303159	44.443559
3504.274837	1054545.346864	44.448564
3504.914623	1054453.954326	44.453569
3504.599767	1054371.682575	44.458573
3504.594905	1054270.271322	44.463578
3504.860739	1054185.394746	44.468583
3504.930939	1054102.669957	44.473588
3504.755658	1053996.268772	44.478593
3504.677592	1053907.684771	44.483597
3504.822511	1053813.760172	44.488602
3504.584858	1053718.161608	44.493607
3504.590714	1053641.707150	44.498612
3504.702094	1053549.229744	44.503617
3504.425520	1053461.924650	44.508621
3504.424143	1053377.465326	44.513626
3504.101517	1053288.333169	44.518631
3504.606773	1053196.749163	44.523636
3504.715066	1053115.160334	44.528641
3504.368797	1053030.463245	44.533645
3504.793971	1052948.723345	44.538650
3504.660801	1052856.660315	44.543655
3504.375122	1052761.245938	44.548660
3504.634722	1052677.311483	44.553665
3504.065703	1052604.794472	44.558669
3504.092672	1052512.699331	44.563674
3504.547690	1052434.129127	44.568679
3504.388822	1052347.654914	44.573684
3504.514691	1052260.360968	44.578689
3504.305543	1052185.657600	44.583693
3505.043106	1052078.201171	44.588698
3504.521850	1051999.689151	44.593703
3504.432255	1051910.592809	44.598708
3504.641889	1051823.567492	44.603713
3504.050440	1051741.880746	44.608717
3504.522873	1051660.789132	44.613722
3504.591428	1051575.326276	44.618727
3504.066919	1051494.878664	44.623732
3504.382911	1051409.854740	44.628737
3503.850262	1051338.472499	44.633741
3504.305774	1051239.533954	44.638746
3504.248053	1051168.842925	44.643751
3503.805103	1051093.970390	44.648756
3504.073488	1051004.896940	44.653761
3504.075464	1050932.360366	44.658765
3503.843348	1050853.880885	44.663770
3503.983891	1050786.528407	44.668775
3504.176601	1050711.738919	44.673780
3504.176336	1050631.481772	44.678785
3503.919263	1050559.754685	44.683789
3504.397289	1050474.110901	44.688794
3504.198052	1050415.781249	44.693799
3504.283424	1050319.877713	44.698804
3504.014505	1050238.308538	44.703809
3504.336190	1050155.772636	44.708813
3504.220793	1050073.403966	44.713818
3503.857390	1050003.230745	44.718823
3504.079111	1049924.373895	44.723828
3504.155282	1049835.216794	44.728833
3503.987404	1049760.763272	44.733837
3503.865728	1049689.870907	44.738842
3503.856564	1049625.712798	44.743847
3503.783107	1049553.363520	44.748852
3503.729346	1049466.537458	44.753857
3503.385975	1049394.134069	44.758861
3503.736578	1049314.861365	44.763866
3503.970622	1049257.220019	44.768871
3503.860235	1049197.994494	44.773876
3503.726466	1049110.114639	44.778881
3503.734732	1049036.876734	44.783885
3503.898908	1048972.296531	44.788890
3503.844130	1048900.418102	44.793895
3503.786441	1048824.775903	44.798900
3503.593923	1048753.979705	44.803905
3503.686559	1048687.285036	44.808909
3503.729509	1048620.018755	44.813914
3503.830612	1048553.900078	44.818919
3503.652279	1048471.421415	44.823924
3503.988571	1048403.042667	44.828929
3503.364871	1048336.558257	44.833933
3503.672254	1048259.014625	44.838938
3503.789700	1048197.231727	44.843943
3503.531317	1048125.859301	44.848948
3504.102521	1048065.447811	44.853953
3503.506019	1048003.201285	44.858957
3503.817820	1047910.789552	44.863962
3503.697061	1047845.374533	44.868967
3503.810506	1047780.499249	44.873972
3503.627367	1047709.881173	44.878977
3503.325616	1047647.003001	44.883981
3503.753790	1047571.167131	44.888986
3503.745946	1047513.837030	44.893991
3503.486571	1047445.930650	44.898996
3503.623011	1047369.753995	44.904001
3503.617473	1047309.911866	44.909005
3504.026217	1047243.244262	44.914010
3503.865808	1047166.631092	44.919015
3503.776112	1047099.271658	44.924020
3503.910267	1047019.036491	44.929025
3503.654557	1046954.405385	44.934029
3503.741349	1046874.658567	44.939034
3503.251724	1046822.130588	44.944039
3503.017184	1046755.176943	44.949044
3503.256745	1046695.384337	44.954049
3503.540352	1046637.514500	44.959053
3503.463704	1046562.809847	44.964058
3503.435306	1046503.928122	44.969063
3503.109412	1046434.475715	44.974068
3503.703055	1046378.965540	44.979073
3503.508083	1046318.757751	44.984077
3503.398845	1046241.447579	44.989082
3503.281810	1046179.873879	44.994087
3503.355025	1046119.716296	44.999092
3503.691037	1046057.970081	45.004097
3503.594634	1046000.445815	45.009101
3503.598598	1045917.705986	45.014106
3503.751834	1045851.063726	45.019111
3503.681275	1045804.732624	45.024116
3503.832787	1045727.951629	45.029121
3503.496755	1045668.628948	45.034125
3503.575286	1045592.244294	45.039130
3503.271462	1045537.742485	45.044135
3503.527189	1045469.147702	45.049140
3503.516212	1045397.602794	45.054145
3503.374118	1045343.265544	45.059149
3503.409463	1045276.732353	45.064154
3503.503982	1045218.299507	45.069159
3503.577651	1045157.455500	45.074164
3503.444063	1045084.671477	45.079169
3503.131478	1045027.752080	45.084173
3503.343804	1044964.758769	45.089178
3503.395044	1044898.990928	45.094183
3503.458604	1044830.902720	45.099188
3503.196907	1044771.751319	45.104193
3503.298721	1044729.728303	45.109197
3503.143014	1044664.957436	45.114202
3503.404528	1044608.518583	45.119207
3503.141125	1044547.047413	45.124212
3503.196409	1044479.728816	45.129217
3502.867365	1044427.151651	45.134221
3503.096670	1044367.528777	45.139226
3503.180405	1044309.088127	45.144231
3503.258725	1044248.716252	45.149236
3503.207728	1044192.034910	45.154241
3502.852972	1044146.702514	45.159245
3503.096158	1044076.837081	45.164250
3503.156142	1044023.322808	45.169255
3503.047379	1043960.660717	45.174260
3503.854819	1043897.364111	45.179265
3503.460182	1043841.508433	45.184269
3503.252816	1043780.792192	45.189274
3503.494213	1043733.909483	45.194279
3503.071920	1043676.801108	45.199284
3503.080509	1043613.536256	45.204289
3503.192157	1043557.594330	45.209293
3503.252501	1043494.705947	45.214298
3502.928756	1043438.351588	45.219303
3503.195422	1043376.393774	45.224308
3503.360792	1043325.366757	45.229313
3503.235094	1043260.574541	45.234317
3503.192786	1043200.211125	45.239322
3503.316487	1043143.007323	45.244327
3503.155383	1043087.395362	45.249332
3503.342071	1043014.531412	45.254337
3503.152467	1042972.349890	45.259341
3503.329866	1042902.770307	45.264346
3503.205079	1042857.196287	45.269351
3503.130971	1042797.606523	45.274356
3503.317058	1042739.712087	45.279361
3502.850450	1042685.015821	45.284365
3503.155387	1042621.304438	45.289370
3503.050578	1042568.672709	45.294375
3502.906988	1042515.950262	45.299380
3503.231820	1042456.097913	45.304385
3502.657694	1042409.338340	45.309389
3503.047861	1042350.536771	45.314394
3502.994298	1042299.053340	45.319399
3503.204915	1042248.781848	45.324404
3503.100864	1042189.770147	45.329409
3502.965247	1042141.969985	45.334413
3503.024904	1042086.987918	45.339418
3503.286419	1042026.948150	45.344423
3502.869331	1041966.536428	45.349428
3503.532426	1041905.173211	45.354433
3503.185349	1041864.555053	45.359437
3503.445538	1041794.754718	45.364442
3503.207406	1041741.750634	45.369447
3503.063328	1041680.614501	45.374452
3503.119491	1041627.657475	45.379457
3502.870335	1041576.972527	45.384461
3503.283662	1041513.810321	45.389466
3502.640168	1041463.285905	45.394471
3502.728213	1041408.775564	45.399476
3502.830546	1041356.484719	45.404481
3502.772327	1041317.940738	45.409485
3502.921498	1041270.859176	45.414490
3503.055829	1041220.107807	45.419495
3502.940699	1041150.747708	45.424500
3503.210306	1041098.716774	45.429505
3502.716610	1041059.566314	45.434509
3503.140977	1040990.791775	45.439514
3502.885466	1040951.697956	45.444519
3502.961304	1040888.874132	45.449524
3503.083656	1040833.386161	45.454529
3502.593824	1040805.056317	45.459533
3502.878140	1040738.910871	45.464538
3503.110907	1040699.541583	45.469543
3502.777591	1040642.000741	45.474548
3502.860606	1040582.361315	45.479553
3502.710227	1040544.503616	45.484557
3503.068306	1040480.372375	45.489562
3502.915241	1040441.354729	45.494567
3502.399241	1040380.748744	45.499572
3502.799441	1040331.588390	45.504577
3502.854410	1040296.787762	45.509581
3502.663397	1040232.550812	45.514586
3503.046737	1040195.859215	45.519591
3502.782733	1040135.305691	45.524596
3502.818414	1040083.303782	45.529601
3502.608099	1040033.274871	45.534605
3502.639359	1039986.008548	45.539610
3502.976465	1039946.133495	45.544615
3502.836146	1039892.709042	45.549620
3502.845757	1039836.069873	45.554625
3502.614997	1039807.208997	45.559629
3502.657522	1039744.184414	45.564634
3502.954099	1039710.790125	45.569639
3502.377054	1039658.981816	45.574644
3502.719540	1039608.664723	45.579649
3502.488917	1039573.713294	45.584653
3502.661043	1039520.620427	45.589658
3502.713433	1039479.919012	45.594663
3502.316432	1039421.119449	45.599668
3502.521536	1039372.659369	45.604673
3502.502526	1039341.731340	45.609677
3502.720936	1039292.398426	45.614682
3502.580017	1039241.191015	45.619687
3502.555452	1039198.083657	45.624692
3502.681751	1039145.768063	45.629697
3502.522806	1039109.448613	45.634701
3502.492483	1039057.737973	45.639706
3502.739905	1039029.180956	45.644711
3502.418131	1038978.677573	45.649716
3502.525149	1038940.863215	45.654721
3502.351996	1038887.821176	45.659725
3502.037152	1038837.605374	45.664730
3502.086750	1038815.846682	45.669735
3502.804031	1038781.894181	45.674740
3502.839374	1038727.462891	45.679745
3502.507857	1038682.565340	45.684749
3502.592104	1038637.405604	45.689754
3502.825299	1038601.308264	45.694759
3502.326609	1038550.443433	45.699764
3502.767232	1038509.670974	45.704769
3502.427092	1038469.993565	45.709773
3502.351715	1038416.254193	45.714778
3502.690931	1038366.313111	45.719783
3502.546892	1038326.699059	45.724788
3502.682984	1038277.854097	45.729793
3502.383192	1038244.065839	45.734797
3502.628507	1038191.238268	45.739802
3502.431921	1038153.758606	45.744807
3502.241506	1038104.965903	45.749812
3502.902899	1038073.628709	45.754817
3502.700343	1038005.307244	45.759821
3502.340838	1037894.275933	45.764826
3502.359768	1037749.629413	45.769831
3502.518825	1037523.445286	45.774836
3502.563560	1037222.330938	45.779841
3502.169572	1036890.230974	45.784845
3502.393784	1036475.419450	45.789850
3502.269019	1036013.629629	45.794855
3502.280340	1035472.172803	45.799860
3502.242357	1034866.147464	45.804865
3502.212642	1034200.844310	45.809869
3502.300275	1033464.322398	45.814874
3502.153479	1032661.256753	45.819879
3501.837876	1031788.994477	45.824884
3501.921890	1030849.055275	45.829889
3501.686368	1029825.063180	45.834893
3501.191548	1028734.297306	45.839898
3501.024608	1027584.177369	45.844903
3500.668294	1026350.918242	45.849908
3500.695083	1025035.436798	45.854913
3500.386058	1023659.603584	45.859917
3500.301448	1022201.369677	45.864922
3499.968326	1020651.535465	45.869927
3499.802655	1019025.187832	45.874932
3499.641573	1017330.439079	45.879937
3499.313576	1015554.830766	45.884941
3499.114074	1013684.255081	45.889946
3499.048407	1011734.159291	45.894951
3498.675353	1009710.753354	45.899956
3498.530261	1007582.569394	45.904961
3497.948974	1005378.482006	45.909965
3498.010906	1003095.209675	45.914970
3497.228223	1000747.502080	45.919975
3497.208330	998294.704498	45.924980
3496.792831	995753.238434	45.929985
3496.187755	993151.897572	45.934989
3495.992565	990466.614257	45.939994
3495.637987	987680.293893	45.944999
3494.875055	984827.284574	45.950004
3494.827274	981865.801755	45.955009
3494.048285	978848.286835	45.960013
3493.612536	975742.217427	45.965018
3492.949478	972557.327662	45.970023
3492.434425	969291.078917	45.975028
3491.893288	965937.587250	45.980033
3491.210635	962526.313430	45.985037
3491.091901	959004.885070	45.990042
3490.529843	955411.334815	45.995047
3489.647491	951812.579668	46.000052
3489.110691	948148.539393	46.005057
3489.004750	944403.349890	46.010061
3487.825981	940571.542577	46.015066
3487.315623	936674.827110	46.020071
3486.642525	932689.789132	46.025076
3486.098867	928613.611065	46.030081
3484.723503	924469.927725	46.035085
3484.552800	920244.511344	46.040090
3483.714000	915946.852450	46.045095
3482.910157	911553.847808	46.050100
3482.032313	907090.404568	46.055105
3481.549888	902546.846906	46.060109
3480.829927	897910.073972	46.065114
3479.987660	893196.993986	46.070119
3478.984007	888399.526185	46.075124
3478.341966	883523.808756	46.080129
3477.070561	878573.244940	46.085133
3476.321707	873528.964990	46.090138
3475.878112	868410.432400	46.095143
3474.968570	863208.009196	46.100148
3474.093437	857913.080251	46.105153
3472.946516	852549.853911	46.110157
3471.969767	847082.170954	46.115162
3470.940842	841553.554095	46.120167
3469.912277	835938.314520	46.125172
3469.202593	830236.331560	46.130177
3467.751542	824453.728339	46.135181
3467.105232	818577.328381	46.140186
3466.150190	812636.431882	46.145191
3465.100854	806597.855662	46.150196
3464.029171	800481.622071	46.155201
3462.593009	794273.413038	46.160205
3461.409201	787981.270385	46.165210
3460.463233	781621.933826	46.170215
3458.582107	775180.333888	46.175220
3458.089252	768645.013548	46.180225
3456.605896	762027.407208	46.185229
3455.428979	755335.670259	46.190234
3454.141467	748562.902419	46.195239
3453.249619	741697.034390	46.200244
3452.086412	734759.918193	46.205249
3450.179177	727741.243956	46.210253
3449.166742	720611.475946	46.215258
3447.664415	713407.300234	46.220263
3446.220194	706132.027742	46.225268
3444.835773	698774.606138	46.230273
3443.464392	691348.093528	46.235277
3442.142727	683814.881595	46.240282
3440.829155	676222.042545	46.245287
3438.956596	668544.460532	46.250292
3437.938718	660778.434026	46.255297
3436.067076	652942.155645	46.260301
3434.362481	645010.476570	46.265306
3432.914908	637022.334620	46.270311
3430.903400	628948.982566	46.275316
3429.471236	620793.944809	46.280321
3428.138593	612570.710913	46.285325
3426.286767	604264.730449	46.290330
3424.554666	595883.812518	46.295335
3422.711668	587432.771862	46.300340
3421.133853	578899.492239	46.305345
3419.182060	570297.920046	46.310349
3417.210958	561620.324537	46.315354
3415.297101	552863.290941	46.320359
3413.808012	544026.582487	46.325364
3412.178275	535129.652653	46.330369
3409.848031	526160.499801	46.335373
3407.808992	517112.755341	46.340378
3405.754625	507988.244917	46.345383
3403.598657	498814.616818	46.350388
3401.932540	489560.161834	46.355393
3399.650699	480245.543546	46.360397
3397.390837	470843.364900	46.365402
3395.299787	461387.186361	46.370407
3392.952426	451875.036186	46.375412
3391.089748	442275.126469	46.380417
3388.541936	432631.455499	46.385421
3386.134821	422918.038163	46.390426
3383.791439	413130.818772	46.395431
3381.103256	403293.718712	46.400436
3379.063971	393385.386580	46.405441
3376.481057	383440.559457	46.410445
3373.836898	373425.828182	46.415450
3371.611955	363350.992963	46.420455
3368.385377	353237.456862	46.425460
3365.891251	343064.523899	46.430465
3363.234047	332843.353933	46.435469
3360.356128	322579.180555	46.440474
3357.373954	312259.218375	46.445479
3354.156907	301910.954322	46.450484
3351.539322	291510.167579	46.455489
3348.244723	281057.023753	46.460493
3345.255119	270568.948216	46.465498
3342.398472	260057.758875	46.470503
3339.235922	249501.195476	46.475508
3335.721279	238897.314035	46.480513
3332.090349	228237.689542	46.485517
3328.869899	217536.063729	46.490522
3325.332221	206872.862038	46.495527
3321.122263	196169.971831	46.500532
3317.336966	185458.975894	46.505537
3313.371065	174734.275064	46.510541
3308.961365	164007.456367	46.515546
3304.895548	153282.498024	46.520551
3300.035447	142553.471053	46.525556
3296.032194	131815.634663	46.530561
3290.832621	121113.026908	46.535565
3285.632030	110421.908483	46.540570
3280.256270	99755.941676	46.545575
3274.355540	89127.556105	46.550580
3267.513623	78542.520910	46.555585
3256.448284	68147.573068	46.560589
3231.931735	58212.208384	46.565594
3205.466669	48577.339597	46.570599
3178.961190	39327.605016	46.575604
3152.942326	30523.235221	46.580609
3127.072016	22254.381186	46.585613
3098.726764	14593.404124	46.590618
3058.693454	7872.696603	46.595623
3006.151430	2245.755592	46.600628
2851.358457	409.251604	46.605633
2697.072381	414.537596	46.610637
2638.886169	409.377104	46.615642
2660.073503	385.768763	46.620647
2722.604107	364.593297	46.625652
2791.987558	363.091093	46.630657
2843.534239	364.274040	46.635661
2870.609932	366.337100	46.640666
2877.354118	361.059805	46.645671
2871.285420	370.995248	46.650676
2860.988531	347.999762	46.655681
2851.269095	357.105928	46.660685
2843.563470	354.213178	46.665690
2839.060352	347.249256	46.670695
2836.447987	364.510324	46.675700
2835.235072	351.798567	46.680705
2833.902493	343.602599	46.685709
2832.377235	332.357505	46.690714
2829.914215	338.755251	46.695719
2827.463946	351.857978	46.700724
2824.709739	337.660994	46.705729
2821.187856	340.664452	46.710733
2817.955627	339.650450	46.715738
2814.887800	328.266428	46.720743
2811.435387	324.661073	46.725748
2808.884656	333.032631	46.730753
2805.681267	338.471842	46.735757
2802.535150	325.394641	46.740762
2799.713836	323.325534	46.745767
2796.142361	327.492659	46.750772
2793.141935	323.758238	46.755777
2789.824383	328.076082	46.760781
2786.287918	322.650940	46.765786
2783.110066	321.133714	46.770791
2779.691130	315.390957	46.775796
2776.979300	315.286834	46.780801
2773.538558	318.240921	46.785805
2769.905517	322.616607	46.790810
2766.830750	319.179773	46.795815
2763.177482	330.374190	46.800820
2760.479544	309.249399	46.805825
2756.918365	311.418891	46.810829
2753.516637	318.286922	46.815834
2750.260440	311.497820	46.820839
2746.433060	320.831150	46.825844
2743.290438	306.856423	46.830849
2740.143038	310.910239	46.835853
2736.758725	306.772389	46.840858
2733.558016	302.834637	46.845863
2729.774504	307.867146	46.850868
2726.452343	308.819762	46.855873
2723.179987	310.012391	46.860877
2719.521808	306.865931	46.865882
2716.690933	303.122634	46.870887
2712.591445	294.158875	46.875892
2709.453715	295.195927	46.880897
2705.821638	299.624257	46.885901
2702.404137	297.206866	46.890906
2699.182101	296.925056	46.895911
2695.882071	288.351594	46.900916
2692.599449	286.260233	46.905921
2688.870653	299.819993	46.910925
2685.056583	299.603640	46.915930
2682.480636	286.750601	46.920935
2678.759391	304.254641	46.925940
2675.184346	300.209537	46.930945
2671.319843	300.415573	46.935949
2667.964372	293.193897	46.940954
2665.086920	291.104309	46.945959
2661.503487	296.587869	46.950964
2658.234480	284.009536	46.955969
2654.795954	290.894116	46.960973
2651.227571	285.546932	46.965978
2648.006575	279.644746	46.970983
2643.371954	292.045278	46.975988
2640.382934	286.987434	46.980993
2637.258459	291.551410	46.985997
2633.900213	282.549642	46.991002
2630.527159	289.830990	46.996007
2626.442451	290.713744	47.001012
2622.825315	277.977271	47.006017
2619.609823	283.275373	47.011021
2616.588465	286.667763	47.016026
2612.844566	289.353333	47.021031
2609.815147	286.797017	47.026036
2606.617806	292.007486	47.031041
2602.454356	291.434027	47.036045
2598.769554	282.185909	47.041050
2595.501872	278.800308	47.046055
2592.232225	299.069956	47.051060
2589.083173	284.909439	47.056065
2585.514994	272.606709	47.061069
2581.556534	283.103065	47.066074
2578.912334	277.694492	47.071079
2574.751310	284.821557	47.076084
2571.674666	263.537110	47.081089
2568.134658	278.033887	47.086093
2564.321425	285.072531	47.091098
2561.367509	275.885745	47.096103
2557.114836	282.464695	47.101108
2553.868548	284.144803	47.106113
2550.523789	281.339310	47.111117
2546.566897	279.782145	47.116122
2543.595009	280.008279	47.121127
2540.343047	282.853190	47.126132
2536.736910	267.771158	47.131137
2533.571365	275.701815	47.136141
2529.841083	277.331713	47.141146
2525.908662	268.769599	47.146151
2522.216316	267.125810	47.151156
2519.617402	263.324820	47.156161
2516.009396	266.422311	47.161165
2512.128293	256.639252	47.166170
2508.518661	259.094459	47.171175
2505.017470	265.746821	47.176180
2501.958018	252.061443	47.181185
2498.516339	263.378669	47.186189
2494.590975	269.014964	47.191194
2491.336562	259.992908	47.196199
2487.841612	261.639758	47.201204
2484.305412	260.898802	47.206209
2480.842355	253.475571	47.211213
2477.425035	266.870851	47.216218
2474.145326	260.079769	47.221223
2470.178442	263.436736	47.226228
2466.886348	259.802563	47.231233
2463.630944	260.619479	47.236237
2460.328322	266.384839	47.241242
2456.674390	260.488738	47.246247
2453.235424	265.940263	47.251252
2449.515030	249.718122	47.256257
2445.683371	265.358018	47.261261
2442.375243	255.797301	47.266266
2439.447668	254.142273	47.271271
2435.410082	261.466872	47.276276
2431.980603	255.966088	47.281281
2428.126241	256.803954	47.286285
2424.763725	263.773153	47.291290
2421.663335	249.932972	47.296295
2418.296336	251.720450	47.301300
2414.943825	258.862229	47.306305
2411.133089	256.981612	47.311309
2407.553639	251.371105	47.316314
2404.291149	257.992128	47.321319
2400.679268	257.169772	47.326324
2397.065166	240.702248	47.331329
2393.717124	244.397695	47.336333
2390.252910	260.115619	47.341338
2386.739482	249.261461	47.346343
2383.073788	256.218419	47.351348
2379.525092	247.091650	47.356353
2376.213021	252.068451	47.361357
2372.643315	246.871506	47.366362
2369.534984	238.590323	47.371367
2365.790551	267.046112	47.376372
2362.414599	237.264725	47.381377
2358.811483	250.612533	47.386381
2355.187554	243.129581	47.391386
2351.782485	252.249243	47.396391
2347.905825	251.945418	47.401396
2344.473710	242.891195	47.406401
2341.326845	249.896971	47.411405
2337.814484	243.182813	47.416410
2334.634584	242.924498	47.421415
2330.469372	246.550721	47.426420
2327.453118	226.926487	47.431425
2323.543588	249.010991	47.436429
2320.177701	248.852712	47.441434
2317.155592	242.804444	47.446439
2313.080403	237.638910	47.451444
2309.564428	245.945296	47.456449
2306.220610	241.872128	47.461453
2302.991354	242.809599	47.466458
2299.331985	239.250884	47.471463
2295.859858	232.911624	47.476468
2292.654386	234.104447	47.481473
2288.882533	240.441130	47.486477
2285.067922	243.442076	47.491482
2281.991304	241.272930	47.496487
2278.311237	245.249604	47.501492
2274.995013	244.729074	47.506497
2271.589137	241.808409	47.511501
2267.894774	245.336090	47.516506
2264.371057	231.363884	47.521511
2260.390050	244.028202	47.526516
2257.474731	244.599691	47.531521
2253.826333	237.013595	47.536525
2250.129583	243.635655	47.541530
2247.187434	228.127151	47.546535
2243.704413	242.509529	47.551540
2240.001152	243.680987	47.556545
2236.182181	235.127588	47.561549
2232.722326	231.146407	47.566554
2229.305511	237.225268	47.571559
2225.826696	235.542469	47.576564
2222.469009	231.117849	47.581569
2218.671727	237.581288	47.586573
2215.504971	237.700981	47.591578
2212.169653	231.624910	47.596583
2208.081639	248.217756	47.601588
2204.868119	240.251950	47.606593
2201.224026	240.158062	47.611597
2197.284591	245.584991	47.616602
2194.475833	232.222989	47.621607
2190.837080	234.860919	47.626612
2187.660817	232.786191	47.631617
2183.879917	237.665179	47.636621
2180.543669	236.199312	47.641626
2177.174787	223.314873	47.646631
2173.124840	246.080913	47.651636
2169.643160	226.498031	47.656641
2166.241406	240.177909	47.661645
2163.007621	220.771392	47.666650
2159.785463	233.704507	47.671655
2156.365501	228.205463	47.676660
2152.603257	213.987374	47.681665
2149.008318	236.122423	47.686669
2145.345659	235.234676	47.691674
2141.854516	221.679040	47.696679
2138.080759	229.959043	47.701684
2134.790236	232.033351	47.706689
2131.344239	233.395847	47.711693
2127.867972	230.090069	47.716698
2124.638617	232.925688	47.721703
2120.888611	237.813618	47.726708
2117.561975	223.855963	47.731713
2113.965580	228.999628	47.736717
2110.365190	237.025618	47.741722
2106.941947	228.816548	47.746727
2102.986746	223.096535	47.751732
2100.021156	207.489005	47.756737
2096.874083	223.692837	47.761741
2093.051169	226.564324	47.766746
2089.623903	211.915929	47.771751
2085.918758	216.365439	47.776756
2082.399836	223.424874	47.781761
2078.723028	219.276232	47.786765
2075.461562	211.255672	47.791770
2071.884727	217.141376	47.796775
2067.794519	226.260198	47.801780
2064.781034	217.655629	47.806785
2061.179922	213.624541	47.811789
2057.928910	225.599354	47.816794
2054.466687	213.441018	47.821799
2050.815275	226.707298	47.826804
2048.038809	218.701748	47.831809
2044.147023	217.666772	47.836813
2040.300286	214.178474	47.841818
2036.990676	216.547205	47.846823
2033.168700	232.311696	47.851828
2030.503184	214.753090	47.856833
2026.653237	213.405387	47.861837
2022.882489	210.032325	47.866842
2019.288718	202.978796	47.871847
2015.684584	219.776583	47.876852
2012.410216	220.574818	47.881857
2009.125928	205.779868	47.886861
2005.418539	213.067240	47.891866
2001.987554	221.259969	47.896871
1998.214884	214.244840	47.901876
1994.760352	214.836029	47.906881
1991.294165	213.746853	47.911885
1987.997814	204.219005	47.916890
1984.502517	215.061405	47.921895
1980.815981	208.794496	47.926900
1977.436570	208.061170	47.931905
1973.747258	201.121889	47.936909
1970.102201	213.928880	47.941914
1967.150252	200.535105	47.946919
1963.706767	210.982921	47.951924
1960.308812	209.245676	47.956929
1956.401720	211.889507	47.961933
1952.831911	222.240378	47.966938
1949.503603	209.854711	47.971943
1945.801836	215.642198	47.976948
1942.753051	210.651482	47.981953
1938.784771	202.664836	47.986957
1934.955595	200.165200	47.991962
1931.830726	209.836226	47.996967
1928.075126	219.158286	48.001972
1925.038893	207.852387	48.006977
1921.576788	214.655376	48.011981
1918.038831	215.669591	48.016986
1914.614950	199.231627	48.021991
1911.221437	206.490240	48.026996
1907.474185	217.288111	48.032001
1903.813719	206.120631	48.037005
1900.418831	207.785961	48.042010
1896.996336	207.332961	48.047015
1893.124234	206.243125	48.052020
1890.055819	208.163095	48.057025
1886.501889	210.406357	48.062029
1882.772765	215.394139	48.067034
1879.250062	208.417359	48.072039
1875.661387	208.395487	48.077044
1872.488948	196.984437	48.082049
1869.069174	207.751669	48.087053
1865.236869	211.901132	48.092058
1861.823621	204.685610	48.097063
1858.604392	216.155542	48.102068
1854.941272	203.819652	48.107073
1851.655697	213.899514	48.112077
1847.915218	215.407408	48.117082
1844.292425	216.534016	48.122087
1840.614453	209.338109	48.127092
1837.184211	212.534921	48.132097
1833.803621	207.125355	48.137101
1830.184700	210.407068	48.142106
1827.376436	201.145853	48.147111
1823.415589	219.536560	48.152116
1819.741433	201.337399	48.157121
1816.484861	198.974505	48.162125
1812.911584	191.979280	48.167130
1809.529655	196.833149	48.172135
1805.507305	195.596886	48.177140
1802.262179	194.701495	48.182145
1799.199603	207.990462	48.187149
1795.920103	204.120341	48.192154
1791.761573	196.295014	48.197159
1787.730756	207.527631	48.202164
1784.866512	203.686767	48.207169
1781.978855	198.986824	48.212173
1777.857606	207.684007	48.217178
1774.562708	192.424912	48.222183
1770.014964	199.739362	48.227188
1767.039428	202.813525	48.232193
1763.739794	203.072740	48.237197
1760.538637	203.319555	48.242202
1757.110778	203.110399	48.247207
1753.221925	207.870062	48.252212
1749.643986	201.593855	48.257217
1746.477259	201.708025	48.262221
1742.628580	212.594319	48.267226
1739.579345	209.131268	48.272231
1736.010903	203.285220	48.277236
1731.878302	197.469422	48.282241
1728.755851	204.313024	48.287245
1725.416811	207.984861	48.292250
1721.918425	198.073484	48.297255
1718.190637	200.039382	48.302260
1715.016430	208.730875	48.307265
1711.628577	195.819484	48.312269
1707.789225	194.336530	48.317274
1704.314856	202.811873	48.322279
1700.452557	199.393822	48.327284
1697.143417	191.022038	48.332289
1694.005023	198.066777	48.337293
1690.276772	203.578266	48.342298
1687.152772	193.651601	48.347303
1683.459208	198.914280	48.352308
1679.764322	205.121614	48.357313
1676.218520	198.954489	48.362317
1672.910127	200.240918	48.367322
1669.646293	192.433976	48.372327
1665.722447	203.270646	48.377332
1661.976946	196.680791	48.382337
1658.840820	193.034610	48.387341
1655.010716	199.608873	48.392346
1652.139450	195.076368	48.397351
1647.906639	198.275770	48.402356
1644.542613	197.111504	48.407361
1641.489334	195.922992	48.412365
1637.544424	193.330254	48.417370
1634.312894	196.742087	48.422375
1630.785219	196.329165	48.427380
1627.185534	193.030702	48.432385
1623.834537	188.613881	48.437389
1620.084809	204.533793	48.442394
1616.644090	190.840560	48.447399
1613.307953	200.575159	48.452404
1609.852442	192.008660	48.457409
1606.254957	194.411664	48.462413
1602.672475	188.809326	48.467418
1599.407347	187.187573	48.472423
1595.473464	202.816166	48.477428
1591.988558	197.025179	48.482433
1588.696079	194.435986	48.487437
1584.687279	196.677010	48.492442
1581.677224	192.500307	48.497447
1578.305189	197.360534	48.502452
1575.338454	206.204000	48.507457
1571.665799	194.098361	48.512461
1567.879131	193.874618	48.517466
1564.155760	191.272591	48.522471
1560.581855	195.620672	48.527476
1557.197879	190.301496	48.532481
1553.397294	194.809914	48.537485
1549.852522	207.902491	48.542490
1546.722440	180.067422	48.547495
1543.266260	193.881637	48.552500
1539.738537	198.451777	48.557505
1536.341677	196.474139	48.562509
1532.244893	191.206120	48.567514
1529.145480	179.840544	48.572519
1525.678695	199.932408	48.577524
1522.061375	191.562353	48.582529
1518.877335	182.288932	48.587533
1515.058163	192.677458	48.592538
1511.685245	176.927685	48.597543
1508.168478	182.995396	48.602548
1504.950669	184.835306	48.607553
1501.310162	191.873106	48.612557
1497.144822	183.755606	48.617562
1494.398214	175.490586	48.622567
1490.647346	194.955718	48.627572
1486.901997	194.567941	48.632577
1483.728037	178.213934	48.637581
1479.973913	182.513755	48.642586
1476.752878	180.853610	48.647591
1472.922051	181.230621	48.652596
1469.415717	183.629498	48.657601
1466.339044	191.500534	48.662605
1462.983536	184.272755	48.667610
1459.408877	181.739870	48.672615
1455.760454	190.069510	48.677620
1451.897218	193.448450	48.682625
1448.353377	182.949856	48.687629
1444.762908	193.327204	48.692634
1441.670509	193.268236	48.697639
1437.817482	184.816187	48.702644
1434.926746	184.954299	48.707649
1431.238073	187.297459	48.712653
1427.353016	183.159688	48.717658
1424.281179	181.078446	48.722663
1420.720634	191.152036	48.727668
1417.153642	177.583175	48.732673
1413.855555	189.069308	48.737677
1409.785827	193.530864	48.742682
1406.680235	184.923603	48.747687
1402.784455	190.139975	48.752692
1399.691543	179.420581	48.757697
1395.997833	182.671037	48.762701
1392.236558	183.206102	48.767706
1388.869541	184.549098	48.772711
1385.660425	181.144377	48.777716
1382.233128	186.974317	48.782721
1378.797614	181.190497	48.787725
1375.105258	185.735989	48.792730
1371.853682	173.821053	48.797735
1367.599016	180.205465	48.802740
1364.410274	180.492733	48.807745
1361.053698	181.301476	48.812749
1357.510746	179.732802	48.817754
1354.104789	172.523086	48.822759
1350.631316	184.999782	48.827764
1347.565374	173.309837	48.832769
1343.542502	180.394439	48.837773
1339.740713	194.808180	48.842778
1336.104159	174.399719	48.847783
1332.900669	174.122266	48.852788
1329.300540	171.930565	48.857793
1326.069219	175.192534	48.862797
1322.728288	183.252557	48.867802
1319.320190	176.661979	48.872807
1315.408903	183.192281	48.877812
1312.048090	174.010116	48.882817
1308.445513	175.597729	48.887821
1304.719625	187.723658	48.892826
1301.397083	182.128015	48.897831
1297.924667	174.494624	48.902836
1294.440929	173.167485	48.907841
1291.174869	175.589529	48.912845
1287.282613	175.225323	48.917850
1283.798397	169.783252	48.922855
1280.678117	181.535451	48.927860
1277.157280	175.182424	48.932865
1273.531130	173.054637	48.937869
1269.411085	179.347427	48.942874
1266.449486	175.637216	48.947879
1262.738110	170.955404	48.952884
1259.288275	177.976038	48.957889
1256.179702	170.300666	48.962893
1252.645101	173.940760	48.967898
1249.398201	173.114391	48.972903
1245.250257	175.512938	48.977908
1241.627272	173.107719	48.982913
1238.495224	181.585727	48.987917
1235.139624	174.256580	48.992922
1231.735857	169.260105	48.997927
1227.785863	178.093140	49.002932
1224.389699	177.724421	49.007937
1220.879584	158.653089	49.012941
1217.317389	179.001482	49.017946
1213.844140	169.950208	49.022951
1210.141887	175.711366	49.027956
1206.849988	173.176730	49.032961
1203.457337	175.007457	49.037965
1199.881329	174.242741	49.042970
1196.554077	173.740920	49.047975
1192.767535	167.505998	49.052980
1189.679736	171.946546	49.057985
1186.056810	168.100095	49.062989
1182.430785	169.543659	49.067994
1178.899531	165.730617	49.072999
1174.818406	165.506373	49.078004
1171.772103	177.619309	49.083009
1168.684794	166.018040	49.088013
1165.132676	164.783944	49.093018
1161.044902	173.261116	49.098023
1157.488574	172.522278	49.103028
1154.223847	174.614556	49.108033
1151.340260	176.823862	49.113037
1147.331763	170.396531	49.118042
1143.782958	172.750386	49.123047
1140.309688	170.966404	49.128052
1136.659024	172.457370	49.133057
1133.549530	167.320421	49.138061
1130.088898	171.384023	49.143066
1126.518694	176.838702	49.148071
1122.751071	175.558717	49.153076
1119.279737	174.840495	49.158081
1115.975533	169.361796	49.163085
1112.197904	174.251494	49.168090
1108.612978	151.886763	49.173095
1104.781354	172.715226	49.178100
1101.688199	169.480135	49.183105
1098.467759	165.368594	49.188109
1094.646334	163.111845	49.193114
1091.608397	168.076346	49.198119
1087.825048	160.944090	49.203124
1084.560780	158.482896	49.208129
1080.787834	168.785930	49.213133
1077.169613	177.727833	49.218138
1073.616691	166.725179	49.223143
1070.279517	176.542024	49.228148
1066.787059	156.874281	49.233153
1063.324828	163.234077	49.238157
1059.789381	175.782075	49.243162
1056.058400	163.094798	49.248167
1052.500281	172.264544	49.253172
1049.238454	161.138478	49.258177
1045.947769	157.649338	49.263181
1042.093117	169.017345	49.268186
1038.971330	168.370100	49.273191
1035.045076	171.242509	49.278196
1031.858989	159.599525	49.283201
1028.234018	160.981434	49.288205
1024.689185	170.639905	49.293210
1021.304542	163.415027	49.298215
1017.683140	168.317452	49.303220
1014.111648	164.027342	49.308225
1011.014073	164.254636	49.313229
1007.290105	170.307153	49.318234
1003.447102	165.376225	49.323239
1000.087449	162.055850	49.328244
996.686128	154.853673	49.333249
993.254956	161.713682	49.338253
989.710384	173.158375	49.343258
986.383344	167.513733	49.348263
982.198488	161.486775	49.353268
979.037283	166.465557	49.358273
975.792820	166.602680	49.363277
972.646110	169.320759	49.368282
969.004038	156.016678	49.373287
964.985205	155.331324	49.378292
961.862424	155.272855	49.383297
958.177546	149.547231	49.388301
954.596561	159.850683	49.393306
951.263537	164.836240	49.398311
947.680724	161.246714	49.403316
944.001210	162.305304	49.408321
940.544966	158.639735	49.413325
937.119702	161.086648	49.418330
933.534681	161.598779	49.423335
929.858389	161.835543	49.428340
926.336247	156.961389	49.433345
923.395600	151.361014	49.438349
919.655576	160.590246	49.443354
916.452760	148.602245	49.448359
912.723982	154.672072	49.453364
909.022182	154.849723	49.458369
905.713731	152.663666	49.463373
902.300940	153.461886	49.468378
898.969208	158.624633	49.473383
895.133298	164.668361	49.478388
891.619790	156.277331	49.483393
887.776845	154.102888	49.488397
884.328690	151.657166	49.493402
880.980224	152.969718	49.498407
877.445381	158.698356	49.503412
873.815050	163.675525	49.508417
870.820415	148.996891	49.513421
866.901426	152.855726	49.518426
863.914468	163.669333	49.523431
860.250075	157.711208	49.528436
856.693508	152.250457	49.533441
853.195943	155.560937	49.538445
849.421754	156.165616	49.543450
845.874472	149.255382	49.548455
842.602813	158.968257	49.553460
838.972294	151.022479	49.558465
835.548635	137.802994	49.563469
831.602268	156.228110	49.568474
828.788920	151.897461	49.573479
825.121069	151.324906	49.578484
821.587122	157.231986	49.583489
818.234974	145.373578	49.588493
814.244233	151.647915	49.593498
811.225290	150.288575	49.598503
807.300164	163.848593	49.603508
804.320447	155.745343	49.608513
800.993721	151.792886	49.613517
796.267462	157.779873	49.618522
793.291011	159.943491	49.623527
790.004037	162.069109	49.628532
786.701515	159.104142	49.633537
783.209127	144.955756	49.638541
779.146209	158.879193	49.643546
776.230163	159.064877	49.648551
772.522613	162.827484	49.653556
768.683333	153.261093	49.658561
765.219091	149.668963	49.663565
761.709030	160.698820	49.668570
758.608089	155.879905	49.673575
754.948626	160.709719	49.678580
751.739530	151.070344	49.683585
748.009027	154.919031	49.688589
744.118072	156.241035	49.693594
740.883083	146.967712	49.698599
737.515851	152.921289	49.703604
733.819060	157.512318	49.708609
730.933340	147.881902	49.713613
726.827797	163.534621	49.718618
723.468606	156.268327	49.723623
719.907377	151.236590	49.728628
716.429870	154.920291	49.733633
713.200759	150.034174	49.738637
709.219543	150.787068	49.743642
705.658973	145.195466	49.748647
702.423205	151.981498	49.753652
699.228378	145.611979	49.758657
695.982792	142.259912	49.763661
692.132999	154.215543	49.768666
688.560965	158.499399	49.773671
684.595886	151.696740	49.778676
681.025265	146.208426	49.783681
677.943741	152.486573	49.788685
674.369372	154.969387	49.793690
670.971089	152.462568	49.798695
667.365025	159.222269	49.803700
663.965444	153.594431	49.808705
660.207412	146.793012	49.813709
656.544108	156.385172	49.818714
653.625577	143.694921	49.823719
649.872303	142.696672	49.828724
646.194743	150.632608	49.833729
643.197203	142.249258	49.838733
639.393116	143.020885	49.843738
635.885175	134.119754	49.848743
631.865730	154.395936	49.853748
628.708355	147.778468	49.858753
625.559487	148.410708	49.863757
621.639984	147.547464	49.868762
618.782758	134.449637	49.873767
615.248555	146.079504	49.878772
611.484541	145.120836	49.883777
607.453867	140.596052	49.888781
603.698490	145.252067	49.893786
600.665711	148.224073	49.898791
597.721606	140.578738	49.903796
593.689261	154.302957	49.908801
590.923757	137.646321	49.913805
586.766156	138.517212	49.918810
583.462860	139.012002	49.923815
579.908220	141.637218	49.928820
576.359759	145.592463	49.933825
572.639910	142.815720	49.938829
569.168351	145.936080	49.943834
565.949305	137.148179	49.948839
562.336993	136.295003	49.953844
558.629224	143.090293	49.958849
555.240664	140.656714	49.963853
551.503997	151.217590	49.968858
548.232323	150.352648	49.973863
544.887784	148.226410	49.978868
541.260898	149.435854	49.983873
538.080097	143.768799	49.988877
534.143500	143.893793	49.993882
530.664157	141.856324	49.998887
527.183122	149.381119	50.003892
523.550398	143.162167	50.008897
520.800291	142.386987	50.013901
516.581082	148.567124	50.018906
513.130881	137.694886	50.023911
509.801815	141.844380	50.028916
505.867228	151.276709	50.033921
502.676918	145.451423	50.038925
499.220658	149.308410	50.043930
495.782816	143.637075	50.048935
492.226095	145.719096	50.053940
488.846398	144.002292	50.058945
485.571678	145.053261	50.063949
481.876581	142.500376	50.068954
478.595799	134.664382	50.073959
474.622161	137.503296	50.078964
471.132261	144.775446	50.083969
467.836764	139.830684	50.088973
464.208520	147.139799	50.093978
460.507652	142.483483	50.098983
457.046862	137.329263	50.103988
453.439883	149.457982	50.108993
450.269365	148.282095	50.113997
446.611851	141.524786	50.119002
443.405340	147.641064	50.124007
439.657215	146.196762	50.129012
435.991395	144.515414	50.134017
432.360612	150.272047	50.139021
428.760731	156.269425	50.144026
425.674555	139.023523	50.149031
422.192718	148.711099	50.154036
418.526084	149.143072	50.159041
415.305962	139.980648	50.164045
411.894917	151.507192	50.169050
408.223128	144.701950	50.174055
404.735757	155.135588	50.179060
400.911090	138.926425	50.184065
397.682961	138.548725	50.189069
393.770403	150.979225	50.194074
390.469539	140.221497	50.199079
387.015072	139.949068	50.204084
383.706564	151.542737	50.209089
380.328992	148.377000	50.214093
376.391895	158.057042	50.219098
373.485697	142.000904	50.224103
369.980811	153.765040	50.229108
365.891071	150.818973	50.234113
362.678719	144.345795	50.239117
358.869559	154.749745	50.244122
355.916328	146.180173	50.249127
351.897436	140.336579	50.254132
347.988578	146.327327	50.259137
344.845904	143.531725	50.264141
341.714716	150.324112	50.269146
338.171209	136.704493	50.274151
334.624819	138.454102	50.279156
331.201620	146.627454	50.284161
327.811177	146.108399	50.289165
323.989993	143.228980	50.294170
320.578507	141.501439	50.299175
317.201382	146.099257	50.304180
313.737552	142.381634	50.309185
310.187254	135.444415	50.314189
306.256452	146.336300	50.319194
302.811516	136.741988	50.324199
299.306163	140.980786	50.329204
295.582292	148.199630	50.334209
292.656535	139.517334	50.339213
289.141600	146.259789	50.344218
285.418398	142.071638	50.349223
281.902638	140.043286	50.354228
278.442489	140.472792	50.359233
275.195356	147.392782	50.364237
271.722380	140.727427	50.369242
268.494759	149.971548	50.374247
264.772905	157.385808	50.379252
260.614706	145.582209	50.384257
257.487093	141.275151	50.389261
253.707490	158.276798	50.394266
250.681723	146.786969	50.399271
247.194398	144.367608	50.404276
243.372399	142.558574	50.409281
240.060959	145.002908	50.414285
236.271767	151.985842	50.419290
232.818597	142.274251	50.424295
229.242024	148.715666	50.429300
225.860280	145.586517	50.434305
222.581747	143.175093	50.439309
219.176782	153.824171	50.444314
215.933433	147.265041	50.449319
212.075487	134.727712	50.454324
208.409859	147.456078	50.459329
205.096646	142.569638	50.464333
201.081740	149.316021	50.469338
198.086174	139.242944	50.474343
194.297892	144.970868	50.479348
190.904099	144.183016	50.484353
187.525030	136.069249	50.489357
183.837106	160.015524	50.494362
180.432911	135.941506	50.499367
177.095043	138.193226	50.504372
173.203319	142.325851	50.509377
169.887613	135.529508	50.514381
166.426880	142.508811	50.519386
163.037723	141.454928	50.524391
159.762410	147.025500	50.529396
155.976920	152.369319	50.534401
152.527981	143.663845	50.539405
148.152704	145.768446	50.544410
145.213884	133.665297	50.549415
141.910663	148.447076	50.554420
138.460159	140.145663	50.559425
134.899928	133.608365	50.564429
131.195632	149.365322	50.569434
128.319053	142.569049	50.574439
124.418887	137.182889	50.579444
120.738609	143.441125	50.584449
117.013246	143.440709	50.589453
113.574033	143.584496	50.594458
110.309657	151.294471	50.599463
107.211556	152.977525	50.604468
103.531171	141.409407	50.609473
100.353311	140.505224	50.614477
96.462292	149.415392	50.619482
92.493040	139.468945	50.624487
89.392446	134.065712	50.629492
86.003032	144.354452	50.634497
82.390673	134.670553	50.639501
78.723237	136.916011	50.644506
75.270377	138.122210	50.649511
71.571672	143.367678	50.654516
68.006218	135.670918	50.659521
64.995605	129.557420	50.664525
61.375921	143.959910	50.669530
57.934468	148.401267	50.674535
54.508590	145.336136	50.679540
50.731597	135.427502	50.684545
47.277806	125.953802	50.689549
43.367302	143.521918	50.694554
40.178268	126.400229	50.699559
37.037105	132.115407	50.704564
33.167588	137.173859	50.709569
29.886375	142.353709	50.714573
26.243674	140.327837	50.719578
22.816697	133.182882	50.724583
19.267749	143.749286	50.729588
15.505154	134.792281	50.734593
12.338349	132.417164	50.739597
8.810361	141.606353	50.744602
5.410022	150.896587	50.749607
1.552432	140.251830	50.754612