Mon Mar 08 18:45:14 2021

Number of Points = 14581

Depth (nm)	Load (N)	Time (s)
-0.172525	102.601538	0.000000
-0.141524	82.994517	0.005005
-0.634440	58.369914	0.010010
-2.184531	14.572138	0.015014
-5.813926	-8.911859	0.020019
-11.041187	-21.035113	0.025024
-16.749616	10.349915	0.030029
-21.106506	-25.492553	0.035034
-25.247559	-11.496452	0.040038
-28.651648	2.484608	0.045043
-31.893139	-5.261048	0.050048
-36.353533	-8.635152	0.055053
-39.634958	-12.011245	0.060058
-43.713497	-1.068420	0.065062
-47.319671	-6.455236	0.070067
-51.181779	-9.065362	0.075072
-54.837932	-10.779565	0.080077
-58.378060	-6.606925	0.085082
-62.532595	-1.052698	0.090086
-66.391668	-13.707891	0.095091
-70.023883	0.465720	0.100096
-73.785545	-6.146701	0.105101
-76.949358	-3.563624	0.110106
-81.030970	-4.590206	0.115110
-84.914882	-10.659586	0.120115
-88.640707	-12.055133	0.125120
-92.907986	-2.203269	0.130125
-96.319778	-5.757171	0.135130
-99.766030	0.124061	0.140134
-103.588071	-6.882355	0.145139
-107.507574	-10.724221	0.150144
-111.737606	-11.004868	0.155149
-114.949046	-21.905757	0.160154
-118.900019	-3.289673	0.165158
-122.664703	-14.207935	0.170163
-126.012111	-8.698812	0.175168
-129.876411	-3.214435	0.180173
-133.602085	-27.398709	0.185178
-137.555508	-21.373436	0.190182
-141.419852	-12.848855	0.195187
-145.229971	-12.767539	0.200192
-149.256392	-4.686983	0.205197
-153.000897	-19.102733	0.210202
-156.762814	-9.422864	0.215206
-160.341094	-16.769257	0.220211
-164.180322	3.749684	0.225216
-168.027334	-10.334320	0.230221
-171.493280	-15.845811	0.235226
-175.526018	-12.889001	0.240230
-179.200596	-8.335211	0.245235
-182.670131	-6.729749	0.250240
-186.621354	-6.671580	0.255245
-190.071843	-9.116945	0.260250
-194.000227	-6.563086	0.265254
-197.630726	-5.513777	0.270259
-201.495717	-5.548187	0.275264
-205.533931	-14.930949	0.280269
-208.978939	-13.889149	0.285274
-213.057915	2.093652	0.290278
-216.865585	-3.240247	0.295283
-220.363458	-9.842489	0.300288
-224.480244	-0.951078	0.305293
-227.826755	-11.190050	0.310298
-231.638795	-0.666333	0.315302
-235.406197	-6.162735	0.320307
-239.017883	-17.158831	0.325312
-243.225257	0.060263	0.330317
-246.880174	-3.889830	0.335322
-250.492365	-5.058849	0.340326
-254.201147	3.109942	0.345331
-258.018192	-5.771901	0.350336
-262.175790	-3.029970	0.355341
-265.481556	-15.963928	0.360346
-269.684800	3.648221	0.365350
-273.347833	3.337277	0.370355
-276.869012	-9.710511	0.375360
-280.536615	4.558916	0.380365
-284.095885	-10.471198	0.385370
-288.163344	-4.676623	0.390374
-291.403767	-5.412944	0.395379
-295.496991	-7.977896	0.400384
-299.520410	-1.031341	0.405389
-303.182985	-8.095994	0.410394
-307.382609	-10.472063	0.415398
-310.873840	-0.153972	0.420403
-314.560438	-4.603496	0.425408
-318.354463	-7.703420	0.430413
-321.880591	-0.364733	0.435418
-325.884034	0.818416	0.440422
-329.064963	-10.285725	0.445427
-332.947274	1.085094	0.450432
-336.941234	-0.560558	0.455437
-340.764084	-16.505647	0.460442
-344.841271	-12.839762	0.465446
-348.824318	5.029622	0.470451
-352.191545	-9.300955	0.475456
-356.069745	-9.219475	0.480461
-359.265421	-7.857744	0.485466
-363.352959	-7.197238	0.490470
-367.185298	-14.911152	0.495475
-370.932706	-9.200655	0.500480
-375.241536	6.748135	0.505485
-378.685948	-8.259165	0.510490
-382.224478	-2.870563	0.515494
-385.698189	-7.456459	0.520499
-389.416713	-11.659505	0.525504
-393.576954	-10.712967	0.530509
-397.211932	-9.036632	0.535514
-401.104193	-10.053479	0.540518
-404.641652	-15.135335	0.545523
-408.187309	-8.871983	0.550528
-412.379623	-6.110062	0.555533
-415.995910	-18.489612	0.560538
-420.202974	-5.223471	0.565542
-424.003753	-9.254066	0.570547
-427.203984	-20.440124	0.575552
-430.957477	-12.637659	0.580557
-434.661683	-20.643135	0.585562
-438.722868	-15.912120	0.590566
-442.493966	-11.497061	0.595571
-446.159194	-7.127285	0.600576
-449.880166	-7.405053	0.605581
-453.449410	-18.532147	0.610586
-457.307702	-17.070781	0.615590
-461.299190	-11.699617	0.620595
-465.096249	-10.956024	0.625600
-468.954263	-5.716540	0.630605
-472.415807	-12.942324	0.635610
-476.437862	-13.113624	0.640614
-480.168694	-3.226946	0.645619
-483.707510	-13.940988	0.650624
-487.637490	-6.384622	0.655629
-491.073298	-12.718834	0.660634
-494.899817	-7.560029	0.665638
-498.946164	-5.299057	0.670643
-502.762576	-12.651034	0.675648
-506.686824	-10.448971	0.680653
-509.924242	-6.147427	0.685658
-513.762475	0.506561	0.690662
-517.335115	-6.430194	0.695667
-521.510310	-16.851733	0.700672
-525.380044	-12.047080	0.705677
-529.129307	-8.732865	0.710682
-532.604872	0.430343	0.715686
-536.068403	-9.720091	0.720691
-539.750407	-13.745814	0.725696
-543.945567	-6.243192	0.730701
-547.784700	-2.785290	0.735706
-551.561602	3.084725	0.740710
-555.409882	-9.796830	0.745715
-558.979129	-6.662701	0.750720
-563.078701	-3.752918	0.755725
-566.488010	-12.945352	0.760730
-570.609883	-5.200518	0.765734
-574.218700	-13.541107	0.770739
-577.516709	2.095161	0.775744
-581.565650	1.266054	0.780749
-585.146050	-22.786078	0.785754
-588.872056	-11.734725	0.790758
-593.103152	-9.625421	0.795763
-596.844093	-8.570483	0.800768
-600.796629	-14.076130	0.805773
-604.306662	-10.795286	0.810778
-608.101833	-5.236062	0.815782
-611.780342	2.037493	0.820787
-614.753575	-10.091253	0.825792
-619.201246	-4.591763	0.830797
-622.829239	-15.975686	0.835802
-626.837780	-8.666733	0.840806
-630.644901	-4.740760	0.845811
-634.191127	-6.424326	0.850816
-637.961860	-4.793743	0.855821
-641.372415	-12.710190	0.860826
-645.572459	-23.255247	0.865830
-649.630958	1.012871	0.870835
-653.211191	-14.267151	0.875840
-656.905882	-2.470116	0.880845
-660.352495	-0.148587	0.885850
-664.448166	-12.845349	0.890854
-668.133798	-11.836981	0.895859
-671.843858	-5.392453	0.900864
-676.089685	11.019821	0.905869
-679.128437	-6.961106	0.910874
-683.184940	-18.271728	0.915878
-687.137195	14.052959	0.920883
-690.501610	-9.282938	0.925888
-694.670696	-5.679048	0.930893
-698.052682	-14.290632	0.935898
-701.888596	3.551027	0.940902
-705.540452	3.847627	0.945907
-709.421462	-13.367917	0.950912
-713.530930	-1.528172	0.955917
-717.210042	-10.674108	0.960922
-720.899962	-10.603198	0.965926
-724.562020	-7.438226	0.970931
-728.198581	-4.919100	0.975936
-731.826381	-8.194715	0.980941
-735.652538	-8.469417	0.985946
-739.527932	-8.387760	0.990950
-743.411369	-2.039988	0.995955
-747.050988	-6.266108	1.000960
-751.162655	-16.080821	1.005965
-754.440569	6.559972	1.010970
-758.170443	-14.134515	1.015974
-762.206874	-4.433536	1.020979
-765.898697	-14.124523	1.025984
-770.068599	-1.857165	1.030989
-773.759662	1.066530	1.035994
-777.097375	-7.988801	1.040998
-780.792789	-5.479112	1.046003
-784.629822	-11.416036	1.051008
-788.717514	15.036175	1.056013
-791.968726	-11.064515	1.061018
-796.008054	-5.092264	1.066022
-799.550617	0.799018	1.071027
-803.243713	-16.277662	1.076032
-807.148613	-0.045829	1.081037
-811.131137	-0.148769	1.086042
-815.026548	-2.802775	1.091046
-818.725424	0.541679	1.096051
-822.619197	-6.675975	1.101056
-826.242580	4.542244	1.106061
-829.628821	-5.681581	1.111066
-833.641167	-3.408136	1.116070
-837.475590	4.989739	1.121075
-841.049173	-12.274706	1.126080
-845.117835	-7.015151	1.131085
-848.856430	4.215209	1.136090
-852.668627	-3.294538	1.141094
-855.915321	-6.906828	1.146099
-859.458248	-21.069742	1.151104
-863.661600	24.627578	1.156109
-867.634763	-14.978396	1.161114
-871.545970	13.829910	1.166118
-875.374998	-30.507518	1.171123
-878.598939	-22.612439	1.176128
-882.755622	20.363680	1.181133
-885.990694	-17.958425	1.186138
-889.917640	14.843421	1.191142
-893.980208	-7.450178	1.196147
-897.286304	-7.170715	1.201152
-901.515128	4.697880	1.206157
-905.037916	-22.182296	1.211162
-908.926512	-6.380251	1.216166
-912.605145	5.811955	1.221171
-916.381994	-14.549902	1.226176
-920.270436	1.550167	1.231181
-923.612292	-11.160985	1.236186
-927.612060	-0.249852	1.241190
-931.638691	-0.826473	1.246195
-934.747399	-16.725420	1.251200
-938.979824	2.512410	1.256205
-942.299980	-11.867332	1.261210
-946.487214	-4.685395	1.266214
-950.659448	7.994196	1.271219
-954.317238	-15.630202	1.276224
-958.199984	-0.291029	1.281229
-961.405376	-1.445164	1.286234
-965.221415	-1.596539	1.291238
-969.023169	-15.907109	1.296243
-972.652886	-28.884352	1.301248
-976.252763	-0.455278	1.306253
-980.128765	-25.965315	1.311258
-984.155323	-0.952823	1.316262
-987.829265	-32.706340	1.321267
-991.540363	6.612884	1.326272
-995.449862	-19.776388	1.331277
-999.166676	6.629416	1.336282
-1003.225226	-16.359984	1.341286
-1006.973019	25.680503	1.346291
-1010.492229	1.551502	1.351296
-1013.920074	-23.295336	1.356301
-1017.984977	-39.580492	1.361306
-1021.559896	13.869163	1.366310
-1025.501898	-4.446154	1.371315
-1029.112120	3.003166	1.376320
-1033.050213	-1.397098	1.381325
-1036.362893	-11.134079	1.386330
-1040.508596	-6.120478	1.391334
-1044.221017	9.568458	1.396339
-1047.901734	-16.527748	1.401344
-1051.979590	4.317575	1.406349
-1055.455513	-8.012409	1.411354
-1059.531848	-8.568243	1.416358
-1063.022973	12.191147	1.421363
-1066.974042	-3.779449	1.426368
-1071.064917	-6.070620	1.431373
-1074.168219	-1.766126	1.436378
-1077.849921	-3.119861	1.441382
-1081.813422	0.462856	1.446387
-1085.756783	-1.946496	1.451392
-1089.432937	-0.237292	1.456397
-1093.024896	-6.706447	1.461402
-1096.935128	-1.593227	1.466406
-1100.750322	-8.906538	1.471411
-1104.566717	-14.221787	1.476416
-1108.630525	-16.723785	1.481421
-1111.816708	-7.063645	1.486426
-1115.524678	2.662631	1.491430
-1119.626442	-6.252608	1.496435
-1123.192716	-13.824879	1.501440
-1127.214700	3.933624	1.506445
-1130.615801	-16.407525	1.511450
-1134.450503	-9.620687	1.516454
-1138.250074	-1.156968	1.521459
-1141.921329	-20.327431	1.526464
-1146.075556	9.008935	1.531469
-1149.628445	-6.747680	1.536474
-1153.460370	-16.655278	1.541478
-1156.842080	0.381133	1.546483
-1160.509961	-9.689888	1.551488
-1165.045036	-10.317213	1.556493
-1168.349345	15.155566	1.561498
-1172.072926	3.671153	1.566502
-1175.975595	-1.336884	1.571507
-1179.620797	-16.949365	1.576512
-1183.495380	0.281047	1.581517
-1186.765948	0.902140	1.586522
-1190.755455	-11.630855	1.591526
-1194.913951	-7.393900	1.596531
-1198.467955	-8.392585	1.601536
-1202.491225	0.416087	1.606541
-1205.931574	-15.659605	1.611546
-1210.119222	-2.945593	1.616550
-1213.461424	-6.972567	1.621555
-1216.967229	-20.637809	1.626560
-1221.185146	8.119117	1.631565
-1224.356408	-28.407070	1.636570
-1229.042894	7.047569	1.641574
-1232.703830	-9.084245	1.646579
-1235.851855	-17.177389	1.651584
-1240.014463	4.090182	1.656589
-1243.454857	-24.912373	1.661594
-1247.233541	-5.368228	1.666598
-1251.176789	-16.986057	1.671603
-1254.750501	-18.478204	1.676608
-1258.955859	12.635730	1.681613
-1262.272482	-34.219079	1.686618
-1266.267053	-2.575969	1.691622
-1269.628229	-4.707615	1.696627
-1273.703228	-12.417409	1.701632
-1277.861333	8.813241	1.706637
-1281.313617	-1.782483	1.711642
-1284.892259	-9.059222	1.716646
-1288.543549	-2.063388	1.721651
-1291.988639	-23.105216	1.726656
-1296.120979	-14.474470	1.731661
-1300.137834	-2.071473	1.736666
-1304.024271	-3.680640	1.741670
-1308.049707	-9.463522	1.746675
-1311.224521	-18.984038	1.751680
-1315.160471	-8.192885	1.756685
-1318.710482	-9.997787	1.761690
-1322.550576	-14.148318	1.766694
-1326.425946	-1.096191	1.771699
-1329.847462	-5.244329	1.776704
-1333.987447	-21.964698	1.781709
-1337.503490	-10.059672	1.786714
-1341.451966	-4.517341	1.791718
-1345.155348	-20.471850	1.796723
-1349.057785	-15.110332	1.801728
-1352.846211	5.870458	1.806733
-1356.458986	-1.165755	1.811738
-1360.046871	-4.478298	1.816742
-1363.795116	-15.947375	1.821747
-1367.473122	-20.771853	1.826752
-1371.622858	-2.584131	1.831757
-1375.300048	-2.220934	1.836762
-1379.022844	-21.196651	1.841766
-1382.885745	-6.140702	1.846771
-1386.201438	-6.820881	1.851776
-1390.310573	-5.503905	1.856781
-1393.890403	-17.094500	1.861786
-1397.947470	-11.752297	1.866790
-1401.782635	-9.908346	1.871795
-1405.139539	-9.263664	1.876800
-1409.221690	-7.824828	1.881805
-1412.602043	-21.095119	1.886810
-1416.568515	-13.752193	1.891814
-1420.213368	-16.662883	1.896819
-1424.045789	-9.428130	1.901824
-1428.233632	-8.265631	1.906829
-1431.622225	-9.467043	1.911834
-1435.410162	-22.990560	1.916838
-1439.660693	2.165684	1.921843
-1442.826467	-40.152687	1.926848
-1446.656084	6.362209	1.931853
-1450.581899	-21.967785	1.936858
-1454.142362	-12.922173	1.941862
-1458.276540	-1.748991	1.946867
-1461.375635	-21.850942	1.951872
-1465.409036	-12.597132	1.956877
-1469.406403	-5.585035	1.961882
-1473.051371	-25.344109	1.966886
-1477.161182	-10.100263	1.971891
-1480.300375	-2.678399	1.976896
-1484.317523	-24.382017	1.981901
-1488.115469	1.564357	1.986906
-1491.810409	-19.241593	1.991910
-1496.009683	10.029967	1.996915
-1499.553303	-14.374483	2.006912
-1500.492180	-5.565619	2.016909
-1497.960807	-8.411813	2.026906
-1495.140720	-4.234123	2.036902
-1493.022294	-5.337441	2.046899
-1491.212919	-12.886677	2.056896
-1489.325223	-4.284136	2.066893
-1487.332947	-14.451979	2.076890
-1485.341607	-4.937665	2.086886
-1483.585449	-0.899050	2.096883
-1481.712747	0.244231	2.106880
-1479.769170	-11.238892	2.116877
-1478.161905	-2.495125	2.126874
-1476.040685	-9.814829	2.136870
-1474.028805	-6.854462	2.146867
-1472.065350	1.519664	2.156864
-1470.368488	-13.608996	2.166861
-1468.251746	-15.154100	2.176858
-1466.444334	-9.459567	2.186854
-1464.740050	-12.640632	2.196851
-1462.950286	-6.848538	2.206848
-1460.782749	-8.646492	2.216845
-1458.583410	-11.204228	2.226842
-1457.311189	-11.797832	2.236838
-1455.333743	-9.638731	2.246835
-1453.080328	-18.676847	2.256832
-1451.072452	-6.648454	2.266829
-1449.507794	-9.298761	2.276826
-1447.721080	-16.765393	2.286822
-1445.757497	-6.730312	2.296819
-1443.803878	-11.915380	2.306816
-1441.988903	-15.919366	2.316813
-1440.085412	-14.302590	2.326810
-1438.337853	-12.041934	2.336806
-1436.638068	-5.384407	2.346803
-1434.269318	-11.294316	2.356800
-1432.574676	-11.336628	2.366797
-1430.852554	-21.394858	2.376794
-1429.086894	-6.271000	2.386790
-1426.708077	-13.848206	2.396787
-1424.847304	-1.816756	2.406784
-1423.081300	-11.379938	2.416781
-1421.290103	-12.909193	2.426778
-1419.474868	-10.727248	2.436774
-1417.521498	-5.182348	2.446771
-1415.486133	-8.403753	2.456768
-1413.935688	-8.271395	2.466765
-1411.951795	-8.745241	2.476762
-1410.092269	-10.279112	2.486758
-1408.276353	-4.017501	2.496755
-1406.301454	-13.811470	2.506752
-1404.365812	-9.035782	2.516749
-1402.412395	-10.488368	2.526746
-1400.469635	-6.681654	2.536742
-1398.842218	-11.092926	2.546739
-1396.980190	-8.826880	2.556736
-1394.778777	-17.654527	2.566733
-1392.960001	-11.735975	2.576730
-1391.586766	-13.664060	2.586726
-1389.680881	-5.983235	2.596723
-1387.251532	-11.193893	2.606720
-1385.375656	-15.059175	2.616717
-1383.905053	-13.690401	2.626714
-1381.520566	-17.597629	2.636710
-1379.942269	-4.325725	2.646707
-1378.236822	-23.248112	2.656704
-1376.331079	-11.391182	2.666701
-1374.099612	-25.088074	2.676698
-1372.573819	-0.181061	2.686694
-1370.523171	-12.060171	2.696691
-1368.652353	-13.954217	2.706688
-1367.002527	-5.493477	2.716685
-1364.783707	-13.142901	2.726682
-1362.892067	-8.772214	2.736678
-1361.292548	-17.565059	2.746675
-1359.244026	-18.646013	2.756672
-1357.492812	-15.315415	2.766669
-1355.513090	-15.382778	2.776666
-1353.834353	-13.990463	2.786662
-1351.702770	-19.173944	2.796659
-1349.947507	-10.873747	2.806656
-1347.839785	-16.271288	2.816653
-1346.033286	-16.225658	2.826650
-1344.223278	-14.162809	2.836646
-1342.637324	-20.272570	2.846643
-1340.655135	-15.204295	2.856640
-1338.566207	-18.631565	2.866637
-1336.560106	-18.084222	2.876634
-1334.928312	-19.338438	2.886630
-1332.868032	-13.253240	2.896627
-1331.379035	-15.703474	2.906624
-1329.220465	-13.769032	2.916621
-1327.215606	-13.541991	2.926618
-1325.384133	-11.968850	2.936614
-1323.631535	-19.731496	2.946611
-1321.678604	-17.288896	2.956608
-1319.759485	-13.421490	2.966605
-1318.094303	-13.856875	2.976602
-1316.173585	-2.599084	2.986598
-1314.192333	-16.137474	2.996595
-1312.525129	-12.225004	3.006592
-1310.383235	-11.276239	3.016589
-1308.646457	-15.419182	3.026586
-1306.691248	-6.339414	3.036582
-1304.931728	-3.515335	3.046579
-1302.892549	-9.692879	3.056576
-1301.020117	-5.176965	3.066573
-1299.015323	-18.749108	3.076570
-1297.507621	-7.572035	3.086566
-1295.574432	-7.425069	3.096563
-1293.662494	-17.600432	3.106560
-1291.565991	-3.326715	3.116557
-1289.671213	-11.732589	3.126554
-1287.893920	-6.277806	3.136550
-1286.174396	-10.556913	3.146547
-1284.227384	-4.327228	3.156544
-1282.213213	-13.450059	3.166541
-1280.644164	-7.335136	3.176538
-1278.474965	-7.996411	3.186534
-1276.833544	-15.373361	3.196531
-1274.800572	-4.146128	3.206528
-1272.507240	-15.138789	3.216525
-1271.253943	-2.387906	3.226522
-1269.475741	-12.505539	3.236518
-1267.361354	-4.022753	3.246515
-1265.552205	-14.720039	3.256512
-1263.317122	-2.887280	3.266509
-1261.526256	-10.123938	3.276506
-1259.747382	-0.366991	3.286502
-1258.041396	-6.653801	3.296499
-1256.025960	1.199081	3.306496
-1254.173507	-10.381398	3.316493
-1252.406666	-7.781069	3.326490
-1250.247731	-0.653738	3.336486
-1248.768488	-7.496329	3.346483
-1246.820368	-3.267202	3.356480
-1244.886331	-10.503076	3.366477
-1242.689289	-3.730766	3.376474
-1241.002352	-8.784583	3.386470
-1239.151128	-14.512019	3.396467
-1237.359699	-9.905726	3.406464
-1235.629926	-10.397175	3.416461
-1233.436838	-5.902517	3.426458
-1231.355215	-11.330520	3.436454
-1229.902533	-9.224608	3.446451
-1227.787859	-14.749470	3.456448
-1225.996249	-6.516556	3.466445
-1224.113806	-2.013229	3.476442
-1222.140551	-10.940005	3.486438
-1220.535947	-6.428532	3.496435
-1218.710857	-7.386774	3.506432
-1216.750761	-12.065886	3.516429
-1214.546600	-6.802497	3.526426
-1212.879054	-5.016729	3.536422
-1211.045439	-7.768335	3.546419
-1209.304286	-13.992845	3.556416
-1207.309341	-4.311479	3.566413
-1205.113708	-12.647017	3.576410
-1203.433889	-0.054327	3.586406
-1201.638337	-13.079796	3.596403
-1199.592691	-3.352853	3.606400
-1197.844688	-6.322843	3.616397
-1195.971713	-11.167989	3.626394
-1194.213922	-14.286376	3.636390
-1192.400935	-2.404947	3.646387
-1190.385088	-5.720930	3.656384
-1188.399462	-8.234750	3.666381
-1186.595568	-12.877793	3.676378
-1184.593063	-4.356497	3.686374
-1183.111819	-3.308225	3.696371
-1181.083386	3.750063	3.706368
-1178.927424	-8.292590	3.716365
-1176.946968	-14.867980	3.726362
-1175.385030	0.397658	3.736358
-1173.420458	-16.110960	3.746355
-1171.663689	-12.326390	3.756352
-1169.606061	-11.480848	3.766349
-1167.903221	-8.687065	3.776346
-1166.069398	-7.093645	3.786342
-1164.154605	-7.613063	3.796339
-1162.274584	-1.667795	3.806336
-1160.296868	-4.906604	3.816333
-1158.488103	-11.441882	3.826330
-1156.515731	-6.493437	3.836326
-1154.670397	-11.127299	3.846323
-1152.809398	-13.886399	3.856320
-1151.032530	-12.108602	3.866317
-1148.925517	-10.077323	3.876314
-1147.138501	-12.631961	3.886310
-1145.484618	-13.122254	3.896307
-1143.905931	-3.146876	3.906304
-1141.425760	-7.411790	3.916301
-1139.407871	-13.784730	3.926298
-1137.824275	-12.347036	3.936294
-1135.956484	-9.183323	3.946291
-1134.254157	-4.913196	3.956288
-1132.208064	-12.440055	3.966285
-1130.125528	-8.153386	3.976282
-1128.477781	-12.400375	3.986278
-1126.452778	-14.620459	3.996275
-1124.706805	-6.864867	4.006272
-1122.677754	-7.819349	4.016269
-1121.031737	-17.819425	4.026266
-1119.060747	-12.310232	4.036262
-1117.314173	-7.744030	4.046259
-1115.088602	-1.789265	4.056256
-1113.443720	-17.225178	4.066253
-1111.732160	-16.733149	4.076250
-1109.564160	-15.963626	4.086246
-1107.660048	-13.596710	4.096243
-1106.153230	-1.183094	4.106240
-1103.924163	-12.402161	4.116237
-1102.165590	-14.731175	4.126234
-1100.285511	-8.665872	4.136230
-1098.530675	-7.691308	4.146227
-1096.585965	-12.982040	4.156224
-1094.652149	-16.338501	4.166221
-1092.825193	-14.882865	4.176218
-1090.663971	-13.090717	4.186214
-1089.133639	-10.408219	4.196211
-1087.339762	-7.437895	4.206208
-1085.185952	-7.670235	4.216205
-1083.066081	-11.245912	4.226202
-1081.376700	-11.844463	4.236198
-1079.884435	-8.571692	4.246195
-1077.716524	-0.735134	4.256192
-1075.999109	-12.023908	4.266189
-1074.295659	-10.644812	4.276186
-1071.798226	-6.066050	4.286182
-1070.284946	-18.619989	4.296179
-1068.512944	-12.553161	4.306176
-1066.512028	-15.789286	4.316173
-1064.609460	-24.704631	4.326170
-1063.238658	-2.799217	4.336166
-1060.742760	-13.835148	4.346163
-1058.774169	-9.332830	4.356160
-1056.847712	-6.742087	4.366157
-1055.064510	-14.918377	4.376154
-1053.321397	-15.929691	4.386150
-1051.791527	-20.381972	4.396147
-1049.819331	-18.690599	4.406144
-1047.636774	-20.064283	4.416141
-1045.592747	-12.558394	4.426138
-1044.196079	-14.900532	4.436134
-1042.325333	-9.207876	4.446131
-1040.183101	-16.311112	4.456128
-1038.460167	-21.774736	4.466125
-1036.418541	-17.715110	4.476122
-1034.507804	-23.688741	4.486118
-1032.813484	-14.928554	4.496115
-1030.851077	-16.232279	4.506112
-1028.790981	-15.592258	4.516109
-1027.142404	-16.627905	4.526106
-1025.250801	-14.116821	4.536102
-1023.430365	-13.425835	4.546099
-1021.337587	-13.364161	4.556096
-1019.397473	-25.714767	4.566093
-1017.941379	-11.609912	4.576090
-1015.980950	-16.874675	4.586086
-1013.985848	-14.899580	4.596083
-1012.087645	-15.990927	4.606080
-1010.400582	-10.399914	4.616077
-1008.277604	-15.539096	4.626074
-1006.354338	-15.464510	4.636070
-1004.590219	-14.358734	4.646067
-1002.742363	-4.778378	4.656064
-1000.462023	-16.526581	4.666061
-998.835468	-12.886831	4.676058
-997.379213	-18.165683	4.686054
-995.363011	-9.917965	4.696051
-993.223953	-10.994133	4.706048
-991.631580	-10.282439	4.716045
-989.611904	-12.034212	4.726042
-987.594207	-15.615570	4.736038
-985.895733	-3.647751	4.746035
-983.722511	-13.569434	4.756032
-981.805007	-12.726577	4.766029
-980.130653	-17.740313	4.776026
-978.713263	-0.381505	4.786022
-976.404697	-3.024158	4.796019
-974.544907	-12.109438	4.806016
-972.694366	-9.579112	4.816013
-970.619940	-3.590559	4.826010
-969.025753	-14.946398	4.836006
-967.287976	-13.369038	4.846003
-965.286266	-19.008237	4.856000
-963.373069	-7.553133	4.865997
-961.163364	-14.847084	4.875994
-959.656870	-11.439146	4.885990
-957.873582	-11.550546	4.895987
-955.977056	-2.712101	4.905984
-953.778229	-6.740795	4.915981
-951.953574	-9.645502	4.925978
-950.121539	-1.739320	4.935974
-948.099538	-4.779785	4.945971
-946.521280	-6.202007	4.955968
-944.481100	-7.428102	4.965965
-942.516118	-11.749376	4.975962
-941.026218	-10.910742	4.985958
-939.182689	-5.542047	4.995955
-937.173892	-4.164306	5.005952
-935.055591	-10.092112	5.015949
-933.135273	-1.404284	5.025946
-931.596610	-4.755855	5.035942
-929.721548	0.617282	5.045939
-927.506966	-7.068982	5.055936
-925.527340	-6.340217	5.065933
-923.867352	-10.405880	5.075930
-922.061615	-2.285481	5.085926
-920.109496	3.656367	5.095923
-918.301168	-4.264921	5.105920
-916.319249	-8.011019	5.115917
-914.676396	-5.447439	5.125914
-912.569975	-8.659258	5.135910
-910.974583	-1.207813	5.145907
-908.880203	-5.600275	5.155904
-906.978463	-10.853993	5.165901
-904.756356	-8.594586	5.175898
-903.208761	-0.551313	5.185894
-901.563829	-4.538771	5.195891
-899.813880	-0.463959	5.205888
-897.460982	-2.189987	5.215885
-895.550874	-16.201423	5.225882
-894.111129	-0.748653	5.235878
-892.056376	-11.780211	5.245875
-890.260590	4.793479	5.255872
-888.279757	-5.176317	5.265869
-886.456119	-9.978609	5.275866
-884.383356	-1.741402	5.285862
-882.605354	-12.963958	5.295859
-880.745236	3.961015	5.305856
-878.689383	-5.967085	5.315853
-877.019780	-5.359232	5.325850
-875.173250	-0.668295	5.335846
-873.245272	-10.735410	5.345843
-871.481609	-1.214102	5.355840
-869.394063	-5.237562	5.365837
-867.465809	-7.047246	5.375834
-865.679003	-5.619744	5.385830
-864.103996	-7.868718	5.395827
-862.156734	-0.522431	5.405824
-859.909945	3.376676	5.415821
-858.125390	2.275199	5.425818
-856.400785	-0.708176	5.435814
-854.392182	7.855096	5.445811
-852.593693	-3.255466	5.455808
-850.769047	-2.697642	5.465805
-848.871409	-4.065071	5.475802
-846.922880	-5.603256	5.485798
-845.227364	-0.897627	5.495795
-843.120966	6.232199	5.505792
-841.339515	-9.334351	5.515789
-839.295325	-1.837757	5.525786
-837.364515	-0.717448	5.535782
-835.958319	1.890336	5.545779
-833.963666	-3.313449	5.555776
-832.064025	2.433192	5.565773
-829.917231	-6.140529	5.575770
-828.123412	0.118795	5.585766
-826.577834	-0.775520	5.595763
-824.443451	-0.169295	5.605760
-822.506639	6.851876	5.615757
-820.556009	-3.354610	5.625754
-819.049251	-12.435455	5.635750
-816.806349	-3.920658	5.645747
-814.911160	-4.465079	5.655744
-813.146973	-10.364601	5.665741
-811.408136	-3.457036	5.675738
-809.734322	-2.991906	5.685734
-807.569705	-2.587857	5.695731
-805.816156	-17.854670	5.705728
-803.929663	-0.089148	5.715725
-801.575339	-7.361873	5.725722
-800.074507	-9.562635	5.735718
-798.201799	-1.305999	5.745715
-796.485334	3.181595	5.755712
-794.579141	1.080246	5.765709
-792.269196	-11.952979	5.775706
-790.624308	-7.570780	5.785702
-788.771096	8.458596	5.795699
-786.988148	-3.333091	5.805696
-785.186159	4.908022	5.815693
-783.180929	-4.113538	5.825690
-780.880124	-9.088330	5.835686
-779.770084	2.342171	5.845683
-777.450132	-10.788954	5.855680
-775.574681	-2.512211	5.865677
-773.825200	0.047062	5.875674
-772.001369	13.340239	5.885670
-770.244061	23.656838	5.895667
-768.089720	-15.522843	5.905664
-766.080642	33.544766	5.915661
-764.444408	3.925814	5.925658
-762.218337	-9.436599	5.935654
-760.836324	5.435012	5.945651
-758.893614	-8.429980	5.955648
-757.133482	27.198616	5.965645
-754.928790	6.117351	5.975642
-753.171491	2.151502	5.985638
-751.209952	5.130038	5.995635
-749.237298	13.299704	6.005632
-747.638051	-0.262515	6.015629
-745.746053	9.268397	6.025626
-743.454706	14.769371	6.035622
-742.128555	5.875307	6.045619
-740.238637	13.796112	6.055616
-738.105148	-1.572448	6.065613
-736.242023	9.164606	6.075610
-734.405523	11.419492	6.085606
-732.730693	-3.987864	6.095603
-730.815243	3.333630	6.105600
-728.426829	6.335543	6.115597
-727.114142	-1.468517	6.125594
-724.604848	0.525709	6.135590
-723.209695	-13.657522	6.145587
-721.384235	15.386240	6.155584
-719.294031	-10.893270	6.165581
-717.373407	-34.316305	6.175578
-715.864987	19.479514	6.185574
-713.826610	2.218890	6.195571
-711.575669	-9.600164	6.205568
-709.900548	-9.108332	6.215565
-708.194103	9.939691	6.225562
-706.359153	2.941087	6.235558
-704.704700	9.192788	6.245555
-702.339037	-25.902906	6.255552
-700.340897	1.021258	6.265549
-698.622671	4.859732	6.275546
-696.895536	12.343977	6.285542
-694.651691	3.176986	6.295539
-693.310427	0.262873	6.305536
-691.328863	6.081807	6.315533
-689.189878	-11.482215	6.325530
-687.784333	3.172541	6.335526
-685.502953	7.037876	6.345523
-683.783216	2.782829	6.355520
-681.895662	8.277336	6.365517
-680.179838	5.136020	6.375514
-678.182981	-0.904797	6.385510
-676.193938	3.720907	6.395507
-674.407546	4.997053	6.405504
-672.462244	3.874766	6.415501
-670.640759	-0.273378	6.425498
-668.666597	5.077834	6.435494
-666.770464	-0.861621	6.445491
-664.908904	5.289127	6.455488
-663.020433	2.486535	6.465485
-660.996210	-3.047086	6.475482
-659.280932	-0.044913	6.485478
-657.550410	4.344232	6.495475
-655.634882	3.498282	6.505472
-653.897564	12.334027	6.515469
-652.019031	-0.832259	6.525466
-649.783163	3.288266	6.535462
-647.874526	-1.611118	6.545459
-646.240317	2.243976	6.555456
-644.432258	-0.550489	6.565453
-642.339582	6.786978	6.575450
-640.854387	4.246194	6.585446
-638.819530	-0.971756	6.595443
-636.474504	0.714090	6.605440
-634.998015	2.909736	6.615437
-633.126218	-10.632804	6.625434
-631.234284	2.820131	6.635430
-629.258822	7.132274	6.645427
-627.735871	-9.589639	6.655424
-625.565144	3.398782	6.665421
-623.705388	-3.916342	6.675418
-621.585269	-3.403965	6.685414
-619.907200	-6.798141	6.695411
-618.063587	-10.316651	6.705408
-616.301768	1.308226	6.715405
-614.234596	0.303879	6.725402
-612.417415	-4.617181	6.735398
-610.632001	-7.834298	6.745395
-608.568190	2.507666	6.755392
-606.754550	7.965100	6.765389
-604.802430	-10.475284	6.775386
-602.984245	-5.708544	6.785382
-601.251582	2.717477	6.795379
-599.517851	-0.224548	6.805376
-597.472535	-1.942198	6.815373
-595.373329	1.568664	6.825370
-593.962072	-10.412983	6.835366
-591.620265	-12.378507	6.845363
-589.672247	3.875899	6.855360
-588.138379	-1.767218	6.865357
-586.336410	-3.867543	6.875354
-584.140330	-1.308418	6.885350
-582.248772	0.370978	6.895347
-580.448878	-8.245014	6.905344
-578.436707	-2.088257	6.915341
-577.041892	-7.222860	6.925338
-575.055893	-5.364344	6.935334
-573.178602	-16.114694	6.945331
-571.246159	-3.966011	6.955328
-569.041856	-14.694388	6.965325
-567.448544	-3.604633	6.975322
-565.559566	-9.872852	6.985318
-563.400106	-11.226618	6.995315
-561.817182	-9.979463	7.005312
-559.841607	-11.540683	7.015309
-557.996681	-10.837457	7.025306
-556.126407	-8.128375	7.035302
-554.283111	-13.437228	7.045299
-552.525447	-11.299075	7.055296
-550.321251	-14.035172	7.065293
-548.794964	-9.921204	7.075290
-546.835776	-9.593045	7.085286
-544.929910	-14.071925	7.095283
-542.993526	-6.017859	7.105280
-541.214478	-12.797423	7.115277
-539.305458	-13.362780	7.125274
-537.275806	-13.129548	7.135270
-535.611799	-6.992929	7.145267
-533.713284	-6.197195	7.155264
-531.536460	-9.794126	7.165261
-529.660676	-1.384593	7.175258
-528.171671	-13.823867	7.185254
-525.934878	-9.024457	7.195251
-524.161604	-4.247320	7.205248
-522.390361	-9.817789	7.215245
-520.715616	-6.194858	7.225242
-518.734683	-1.447726	7.235238
-516.647977	-5.173929	7.245235
-515.012327	-0.941619	7.255232
-512.974769	-9.653943	7.265229
-511.066408	-11.027555	7.275226
-509.280112	-7.310332	7.285222
-507.207674	-6.318155	7.295219
-505.579886	-14.467681	7.305216
-503.548878	0.434670	7.315213
-501.814368	-13.911608	7.325210
-499.732248	-13.940922	7.335206
-497.965165	-5.351379	7.345203
-495.842585	-6.615515	7.355200
-494.544343	-10.934162	7.365197
-492.499046	-6.399383	7.375194
-490.481142	-8.044673	7.385190
-488.364224	-5.438080	7.395187
-486.701836	-8.120748	7.405184
-484.980928	-11.305369	7.415181
-482.937060	-8.044504	7.425178
-481.122459	-11.117775	7.435174
-479.129643	-13.651111	7.445171
-477.439310	-7.078146	7.455168
-475.608778	-12.138601	7.465165
-473.457448	-2.538345	7.475162
-471.687533	-12.376261	7.485158
-469.580460	-7.846591	7.495155
-468.102012	-6.907935	7.505152
-466.186620	-15.469664	7.515149
-464.244151	-7.476497	7.525146
-462.418451	-23.291448	7.535142
-460.438891	-12.643804	7.545139
-458.432150	-14.974094	7.555136
-456.686794	-10.549273	7.565133
-454.972637	-13.912786	7.575130
-452.863142	-8.961929	7.585126
-450.757642	-16.271960	7.595123
-449.107183	-14.831839	7.605120
-447.294003	-8.903702	7.615117
-445.444097	-13.278840	7.625114
-443.533927	-13.416430	7.635110
-441.935942	-10.693773	7.645107
-439.868507	-4.138365	7.655104
-437.781956	-13.025815	7.665101
-436.094525	-2.449907	7.675098
-434.160706	-12.493964	7.685094
-432.281462	0.193851	7.695091
-430.509250	-3.692052	7.705088
-428.687207	-12.017809	7.715085
-426.646216	-7.930684	7.725082
-424.859939	-19.539517	7.735078
-422.675071	-4.349040	7.745075
-420.990017	-9.463592	7.755072
-419.179634	-8.491070	7.765069
-416.947259	-8.796924	7.775066
-415.691129	-10.558925	7.785062
-413.769046	-4.802877	7.795059
-411.592737	2.823021	7.805056
-409.673416	-3.066267	7.815053
-407.967922	-14.396944	7.825050
-406.075506	-7.608307	7.835046
-404.171624	-7.127522	7.845043
-402.387094	-5.817716	7.855040
-400.428439	-17.201439	7.865037
-398.255843	-13.403712	7.875034
-396.471351	-11.912325	7.885030
-394.911143	-9.856204	7.895027
-392.864422	-18.535160	7.905024
-391.117916	-8.371265	7.915021
-389.150088	-3.996121	7.925018
-387.326759	-9.705860	7.935014
-385.471878	-11.733962	7.945011
-383.364721	-2.728114	7.955008
-381.744337	-5.853986	7.965005
-379.782326	-8.371272	7.975002
-377.675532	-12.149511	7.984998
-375.671380	-6.142861	7.994995
-374.553272	-18.685464	8.004992
-372.633201	0.854517	8.014989
-370.152695	-7.863686	8.024986
-368.234637	-8.449297	8.034982
-366.507455	-13.829474	8.044979
-364.733240	-7.122978	8.054976
-362.902373	-5.351614	8.064973
-361.213015	-3.548182	8.074970
-359.475337	-6.309099	8.084966
-357.238640	-9.138630	8.094963
-355.154761	-2.143683	8.104960
-353.517271	-3.691813	8.114957
-351.607770	-5.641772	8.124954
-349.499493	-8.515529	8.134950
-347.973202	-5.669259	8.144947
-346.104152	-1.346198	8.154944
-343.942853	-3.544762	8.164941
-342.214706	4.812723	8.174938
-340.364021	-5.800607	8.184934
-338.564709	-13.289027	8.194931
-336.667257	-1.546621	8.204928
-334.731995	-6.609487	8.214925
-333.107463	-10.190705	8.224922
-330.731226	-6.832771	8.234918
-328.992363	-13.215795	8.244915
-327.263919	-7.455602	8.254912
-325.516238	-0.165387	8.264909
-323.460916	-6.723660	8.274906
-321.497537	-12.416238	8.284902
-319.736365	-5.840248	8.294899
-317.949714	-3.512341	8.304896
-315.830066	-8.072545	8.314893
-314.138864	-0.770148	8.324890
-312.237061	-13.458363	8.334886
-310.272247	-2.681906	8.344883
-308.562062	-11.772849	8.354880
-306.738957	1.745060	8.364877
-304.799601	-5.162566	8.374874
-302.796704	-10.237783	8.384870
-300.797593	-13.206171	8.394867
-299.058211	-3.828917	8.404864
-297.334239	-5.390814	8.414861
-295.341856	-5.392996	8.424858
-293.555276	-11.025754	8.434854
-291.364586	-2.479971	8.444851
-289.636811	-5.971858	8.454848
-287.845506	-12.513220	8.464845
-286.012337	-3.989309	8.474842
-284.091248	-6.040535	8.484838
-282.127925	-13.193535	8.494835
-280.468409	-8.701193	8.504832
-278.599314	-1.731886	8.514829
-276.616064	-5.847148	8.524826
-274.346716	-13.053725	8.534822
-272.999290	-3.904401	8.544819
-271.075143	-5.390867	8.554816
-269.202172	-4.087182	8.564813
-266.948932	-9.987030	8.574810
-265.290552	-5.930265	8.584807
-263.649722	0.227632	8.594803
-261.458170	-15.056684	8.604800
-259.359989	4.505514	8.614797
-257.883999	-10.456181	8.624794
-256.104757	-11.543734	8.634791
-254.184210	-13.324862	8.644787
-252.005970	-11.877265	8.654784
-250.339285	-12.754226	8.664781
-248.386352	-8.292903	8.674778
-246.435195	-2.320306	8.684775
-244.792396	-14.723992	8.694771
-242.896478	-7.141598	8.704768
-240.836003	-9.701331	8.714765
-238.994447	-11.641937	8.724762
-237.207960	-0.009617	8.734759
-235.343047	-7.827375	8.744755
-233.412175	-11.294797	8.754752
-231.615168	-8.125356	8.764749
-229.834239	3.496808	8.774746
-227.082231	-19.944992	8.784743
-226.028044	-24.458226	8.794739
-224.166216	-12.638990	8.804736
-222.003103	-13.262017	8.814733
-220.071192	-13.095018	8.824730
-218.535297	-20.020287	8.834727
-216.710664	-13.010680	8.844723
-214.542246	-19.027990	8.854720
-212.874719	-9.408685	8.864717
-210.650903	-3.585357	8.874714
-208.858667	-17.241236	8.884711
-207.229758	-16.465371	8.894707
-205.351487	-19.333875	8.904704
-203.320716	-10.329875	8.914701
-201.530027	-14.128570	8.924698
-199.577513	-17.725728	8.934695
-198.017056	-11.199713	8.944691
-195.806522	-15.534330	8.954688
-194.087925	-16.678473	8.964685
-192.369765	-19.578256	8.974682
-190.112325	-24.907150	8.984679
-188.129791	-32.014192	8.994675
-186.695746	-20.232447	9.004672
-184.573538	-10.684099	9.014669
-182.695383	-21.467481	9.024666
-180.770389	-18.518945	9.034663
-179.053183	-23.387426	9.044659
-177.204765	-17.213653	9.054656
-175.362414	-21.440552	9.064653
-173.299759	-13.404730	9.074650
-171.781844	-21.695989	9.084647
-169.731543	-23.076195	9.094643
-167.674056	-16.889988	9.104640
-165.945666	-16.352590	9.114637
-164.000222	-19.470193	9.124634
-161.909044	-18.788587	9.134631
-160.074211	-16.202998	9.144627
-158.593839	-16.464403	9.154624
-156.550664	-21.457512	9.164621
-154.723667	-22.838388	9.174618
-152.579357	-17.755447	9.184615
-150.574587	-25.777025	9.194611
-149.099470	-19.137892	9.204608
-147.291800	-25.440197	9.214605
-145.434321	-15.124868	9.224602
-143.291344	-26.198360	9.234599
-141.601458	-22.059698	9.244595
-139.678031	-17.037811	9.254592
-137.539385	-21.405114	9.264589
-135.839721	-16.011219	9.274586
-133.870838	-17.135258	9.284583
-132.233273	-14.543433	9.294579
-130.145857	-11.066583	9.304576
-128.488860	-12.069805	9.314573
-126.463828	-10.949736	9.324570
-124.285668	-15.939098	9.334567
-122.670264	-7.819232	9.344563
-121.154711	-12.863916	9.354560
-119.054796	-10.870038	9.364557
-116.996272	-14.853506	9.374554
-115.256585	-8.313396	9.384551
-113.427686	0.582383	9.394547
-111.172994	-10.775751	9.404544
-109.571688	-6.826603	9.414541
-107.954515	1.346679	9.424538
-105.617856	-7.612000	9.434535
-103.896990	-10.381110	9.444531
-102.269036	-0.019639	9.454528
-100.000153	-8.032802	9.464525
-98.508078	-6.570323	9.474522
-96.463758	-15.550241	9.484519
-94.363742	-9.419693	9.494515
-92.625058	-8.264963	9.504512
-91.185861	-12.501693	9.514509
-89.248738	-1.313259	9.524506
-86.849889	-5.764667	9.534503
-85.149342	-12.978227	9.544499
-83.326495	-9.004408	9.554496
-81.634760	-7.707975	9.564493
-79.346473	-13.880082	9.574490
-77.712280	-12.501839	9.584487
-75.810831	-9.581035	9.594483
-73.876117	-21.409114	9.604480
-71.996210	-10.323644	9.614477
-70.405154	-9.757952	9.624474
-68.363204	-10.794126	9.634471
-66.446777	-13.168110	9.644467
-64.250939	-17.629737	9.654464
-63.132683	-7.917950	9.664461
-60.755282	-18.443018	9.674458
-58.769734	-11.162120	9.684455
-56.993369	-9.885486	9.694451
-55.137354	-13.809758	9.704448
-53.257813	-16.495202	9.714445
-51.643753	-14.820058	9.724442
-49.542787	-9.030658	9.734439
-47.688545	-1.510913	9.744435
-45.784842	-8.707913	9.754432
-44.004199	-9.959740	9.764429
-42.019785	-20.224741	9.774426
-40.162676	-11.972853	9.784423
-38.136189	-3.601142	9.794419
-36.425240	-4.732903	9.804416
-34.666114	-10.039016	9.814413
-32.770939	-5.255674	9.824410
-30.591527	-7.308440	9.834407
-28.888902	-12.873944	9.844403
-27.201826	-4.675441	9.854400
-25.268664	-6.917859	9.864397
-23.332799	1.526743	9.874394
-21.329406	-9.991752	9.884391
-19.481585	-5.646091	9.894387
-17.462897	-8.309496	9.904384
-15.616340	-8.108194	9.914381
-13.898339	-2.276618	9.924378
-12.246033	-17.267901	9.934375
-10.209714	-8.390914	9.944371
-8.336619	-10.156388	9.954368
-6.297229	-15.668230	9.964365
-4.588729	-7.541019	9.974362
-3.401997	-0.053707	9.984359
-2.006775	44.172592	9.994355
-0.701276	107.645837	10.004352
0.000000	157.638680	10.009357
0.946778	191.087915	10.014362
1.709614	230.831544	10.019367
2.041170	255.266222	10.024371
2.714293	267.744071	10.029376
2.457382	299.056477	10.034381
2.803830	334.062004	10.039386
3.268500	327.382296	10.044391
3.108552	354.123695	10.049395
3.595425	344.483746	10.054400
3.615891	360.471882	10.059405
3.903875	368.715766	10.064410
3.979607	378.277110	10.069415
3.548062	380.902144	10.074419
3.743367	390.904880	10.079424
3.753431	390.748777	10.084429
3.981648	386.472115	10.089434
3.999613	389.069606	10.094439
4.196948	395.998633	10.099443
4.385546	390.394227	10.104448
4.321268	401.028137	10.109453
4.520957	400.707751	10.114458
4.316760	397.548700	10.119463
4.338846	423.354471	10.124467
4.775623	413.541122	10.129472
4.796407	427.821490	10.134477
4.532840	411.537828	10.139482
4.445870	412.374884	10.144487
4.294133	427.901719	10.149491
4.984307	431.741834	10.154496
4.585499	448.571205	10.159501
4.752298	441.637765	10.164506
5.054121	443.642801	10.169511
4.769106	432.858074	10.174515
4.900859	443.438672	10.179520
4.739019	454.636948	10.184525
4.863852	442.569466	10.189530
4.969926	438.064696	10.194535
4.863478	458.597341	10.199539
5.182634	449.066074	10.204544
5.195342	453.495210	10.209549
5.177959	455.658392	10.214554
5.511297	454.091427	10.219559
5.032440	469.490714	10.224563
5.300618	458.665041	10.229568
5.402428	469.209433	10.234573
5.510032	466.068442	10.239578
5.440082	485.294349	10.244583
5.463964	502.244015	10.249587
5.792533	487.043780	10.254592
5.480589	499.877641	10.259597
5.771560	502.374838	10.264602
6.030465	505.600956	10.269607
5.707429	507.016554	10.274611
5.984277	501.462682	10.279616
5.909728	505.566714	10.284621
5.919601	508.156056	10.289626
5.956045	508.525588	10.294631
5.928461	510.192099	10.299635
5.999569	499.763673	10.304640
6.012303	528.696575	10.309645
6.008172	494.826626	10.314650
6.103358	515.409191	10.319655
5.832507	522.428724	10.324659
5.966253	520.174511	10.329664
6.216771	523.837201	10.334669
5.957537	520.617516	10.339674
5.754366	520.807653	10.344679
6.035405	532.219195	10.349683
6.336115	544.505954	10.354688
5.810938	551.545566	10.359693
6.072194	549.982204	10.364698
6.592618	555.789044	10.369703
6.213277	562.748632	10.374707
6.791967	567.402913	10.379712
7.093113	588.848425	10.384717
6.600890	580.312221	10.389722
6.496220	574.833366	10.394727
6.516502	598.465156	10.399731
6.840089	592.044369	10.404736
6.795134	599.168256	10.409741
6.765652	606.163523	10.414746
7.220330	591.329412	10.419751
6.836063	603.296551	10.424755
7.012406	600.313298	10.429760
6.772110	606.438610	10.434765
7.131819	602.965647	10.439770
7.035840	610.088215	10.444775
7.153767	634.257991	10.449779
7.309645	632.831274	10.454784
7.116923	641.730722	10.459789
7.371222	645.802842	10.464794
7.504272	643.378413	10.469799
7.104521	641.989856	10.474803
7.416334	646.048072	10.479808
7.508320	666.573016	10.484813
7.500021	645.153296	10.489818
7.430210	651.896400	10.494823
7.546487	652.795669	10.499827
7.877924	665.164361	10.504832
7.965110	689.280786	10.509837
7.803153	683.470408	10.514842
8.042477	672.193444	10.519847
7.915849	685.256528	10.524851
8.298247	680.543608	10.529856
8.050076	681.415853	10.534861
8.295748	661.748578	10.539866
7.984818	660.765317	10.544871
8.028361	693.331624	10.549875
8.537283	688.354095	10.554880
8.223947	686.106512	10.559885
8.173768	682.736753	10.564890
8.626266	703.120669	10.569895
8.502799	696.667064	10.574899
8.496275	692.192790	10.579904
8.547393	693.648075	10.584909
8.401055	686.259843	10.589914
8.482018	696.489185	10.594919
8.488539	696.794110	10.599923
8.787588	688.290905	10.604928
8.751674	691.532549	10.609933
8.634656	693.714812	10.614938
9.206931	700.741878	10.619943
8.664457	699.611043	10.624947
8.553714	711.920994	10.629952
8.778413	703.169444	10.634957
8.608513	709.392380	10.639962
9.026974	695.447027	10.644967
8.626738	703.375100	10.649971
8.893014	704.031252	10.654976
9.000985	707.700956	10.659981
9.085033	732.891850	10.664986
9.288638	736.469037	10.669991
9.068480	730.483421	10.674995
9.291264	734.451785	10.680000
9.233646	750.943235	10.685005
9.368530	734.698157	10.690010
9.431038	737.302798	10.695015
9.006213	741.989465	10.700019
9.331425	744.161124	10.705024
9.221926	752.131160	10.710029
9.169022	747.981233	10.715034
9.418325	749.811765	10.720039
9.313667	783.581466	10.725043
9.641853	781.247315	10.730048
9.732446	784.251184	10.735053
9.763853	779.983721	10.740058
9.976469	783.406519	10.745063
9.901195	782.470818	10.750067
9.974575	782.102762	10.755072
9.837205	779.532208	10.760077
9.879330	787.249422	10.765082
10.031339	788.010536	10.770087
9.941923	785.184752	10.775091
10.089352	789.202996	10.780096
9.944155	803.399820	10.785101
10.126409	807.421977	10.790106
10.708375	809.593695	10.795111
10.253750	820.154554	10.800115
10.700784	808.331845	10.805120
10.617738	827.760568	10.810125
10.508843	827.451546	10.815130
10.261310	815.078870	10.820135
10.502119	817.511585	10.825139
10.719126	821.648051	10.830144
10.686483	833.431561	10.835149
10.657562	813.804724	10.840154
10.881063	820.373391	10.845159
10.866461	818.320990	10.850163
11.120451	821.647312	10.855168
11.000150	830.027544	10.860173
10.914874	827.065473	10.865178
11.069641	828.557856	10.870183
10.962511	842.753378	10.875187
11.245778	821.354703	10.880192
11.027609	830.758219	10.885197
11.271991	833.914187	10.890202
11.476964	819.469756	10.895207
11.327504	829.079932	10.900211
11.106238	827.221341	10.905216
11.101414	833.670313	10.910221
10.914221	835.411204	10.915226
11.210323	827.698442	10.920231
11.428567	839.779410	10.925235
11.378958	825.727239	10.930240
11.360500	839.336181	10.935245
11.509273	848.682758	10.940250
11.915994	843.948561	10.945255
11.614668	861.535567	10.950259
11.633674	866.239792	10.955264
11.868602	857.951720	10.960269
11.932383	859.857589	10.965274
11.773638	863.899457	10.970279
11.441630	880.113118	10.975283
11.744947	874.971202	10.980288
11.998364	870.576839	10.985293
11.548821	859.931575	10.990298
12.135948	866.565268	10.995303
11.746585	873.958688	11.000307
12.103388	865.091352	11.005312
12.177496	862.394013	11.010317
11.901444	867.457537	11.015322
12.281291	889.944351	11.020327
12.269665	904.244549	11.025331
12.650538	889.590643	11.030336
12.554711	903.839615	11.035341
12.330940	900.864925	11.040346
12.842637	901.526098	11.045351
12.359966	918.981248	11.050355
12.423454	905.377743	11.055360
12.509197	899.778507	11.060365
12.373299	906.018181	11.065370
12.339469	906.100887	11.070375
12.504568	922.620087	11.075379
12.906767	901.426254	11.080384
12.734972	921.556812	11.085389
12.690461	919.414549	11.090394
13.394858	907.911836	11.095399
12.857827	896.052046	11.100403
12.647696	914.135506	11.105408
13.158713	924.419419	11.110413
13.152524	920.664117	11.115418
13.207625	922.222869	11.120423
13.158978	936.164725	11.125427
13.419014	934.018041	11.130432
13.224420	939.603188	11.135437
13.333181	939.626881	11.140442
13.355227	933.589934	11.145447
13.106620	943.700127	11.150451
13.346078	934.687461	11.155456
13.369498	924.114948	11.160461
13.624594	934.362417	11.165466
13.869585	935.376793	11.170471
13.447222	932.629314	11.175475
13.474789	937.862057	11.180480
13.856157	934.735649	11.185485
14.005267	926.394993	11.190490
13.903979	936.645688	11.195495
13.861518	939.986204	11.200499
14.185630	935.252538	11.205504
14.063706	941.180913	11.210509
14.045455	932.384396	11.215514
14.362353	933.672733	11.220519
13.963102	941.310616	11.225523
14.350383	936.590529	11.230528
14.383791	926.838019	11.235533
13.818337	938.400666	11.240538
14.292220	930.094941	11.245543
13.892617	924.767074	11.250547
13.896256	941.711021	11.255552
14.316530	958.180101	11.260557
14.284160	965.866714	11.265562
14.600251	959.789165	11.270567
14.434916	961.537623	11.275571
14.694004	960.830857	11.280576
14.609361	963.041113	11.285581
14.458814	965.701854	11.290586
14.761589	963.846395	11.295591
14.675846	970.177446	11.300595
15.007528	951.522669	11.305600
14.856726	972.977756	11.310605
14.890354	970.255314	11.315610
15.548162	954.499026	11.320615
15.113136	958.655949	11.325619
15.333097	958.327589	11.330624
15.159132	968.242965	11.335629
14.989228	960.959277	11.340634
15.572686	962.130985	11.345639
15.326338	961.448064	11.350643
15.420564	949.135882	11.355648
15.203966	954.920089	11.360653
15.313029	961.852430	11.365658
15.261076	968.529754	11.370663
15.092702	965.065239	11.375667
15.339645	955.762782	11.380672
15.305125	956.889550	11.385677
15.336340	957.824483	11.390682
15.642680	964.069341	11.395687
15.256456	961.781298	11.400691
15.469853	952.990400	11.405696
15.379491	967.547649	11.410701
15.653361	980.036182	11.415706
16.096459	979.112408	11.420711
15.890323	993.588799	11.425715
16.149431	984.267037	11.430720
16.070635	987.433584	11.435725
15.840178	984.762721	11.440730
16.247754	984.890144	11.445735
16.124845	1000.897123	11.450739
15.899207	1005.651452	11.455744
16.078806	990.390872	11.460749
16.021804	991.218451	11.465754
16.429450	985.104211	11.470759
16.178820	999.497818	11.475763
16.103727	989.691608	11.480768
16.405195	994.730873	11.485773
16.194245	996.865084	11.490778
16.395960	988.594851	11.495783
16.428717	995.783809	11.500787
16.400071	985.555450	11.505792
16.064559	1000.924549	11.510797
16.309066	1000.224838	11.515802
16.504362	994.317930	11.520807
16.741008	1032.529722	11.525811
17.106279	1034.171482	11.530816
17.186528	1022.173709	11.535821
17.203363	1026.487242	11.540826
16.983749	1008.611036	11.545831
17.091866	1004.706592	11.550835
17.263821	982.622104	11.555840
16.745173	993.201183	11.560845
16.799340	997.404674	11.565850
17.426521	1010.885569	11.570855
17.146760	1015.415141	11.575859
17.136832	1012.415782	11.580864
17.327446	1017.286654	11.585869
17.361038	1037.938133	11.590874
17.682784	1011.029395	11.595879
17.071227	1029.834623	11.600883
17.538036	1011.401070	11.605888
17.215161	1032.164591	11.610893
17.563917	1026.922332	11.615898
17.589651	1010.388422	11.620903
17.340931	1016.975725	11.625907
17.662786	1030.401256	11.630912
17.844714	1025.116220	11.635917
17.751525	1018.181395	11.640922
17.676593	1008.130716	11.645927
17.487782	1027.034096	11.650931
17.655067	1023.071323	11.655936
17.733243	1022.806578	11.660941
17.498504	1014.345742	11.665946
18.009432	1016.202391	11.670951
17.774002	1039.468825	11.675955
17.905389	1045.716391	11.680960
18.063171	1035.289526	11.685965
17.752652	1045.920605	11.690970
18.003532	1034.343469	11.695975
17.987618	1050.232510	11.700979
18.085390	1050.958134	11.705984
18.418417	1038.867990	11.710989
17.742467	1052.145176	11.715994
18.599127	1066.478938	11.720999
18.444416	1063.168341	11.726003
18.801945	1091.274653	11.731008
19.056210	1070.889505	11.736013
18.812731	1056.030655	11.741018
18.889680	1039.217304	11.746023
18.561757	1057.805438	11.751027
18.947618	1030.711393	11.756032
18.582452	1044.366364	11.761037
18.507537	1056.379152	11.766042
18.932353	1047.579708	11.771047
18.977309	1090.285072	11.776051
19.060570	1063.907869	11.781056
19.064438	1097.687802	11.786061
18.910487	1064.997922	11.791066
19.440853	1086.502233	11.796071
19.111215	1075.779336	11.801075
19.141969	1067.594674	11.806080
19.381467	1085.538823	11.811085
18.960328	1063.727006	11.816090
19.449704	1088.429663	11.821095
19.457188	1068.866061	11.826099
19.628842	1081.605956	11.831104
19.557486	1077.179751	11.836109
19.424376	1071.820363	11.841114
19.615951	1070.331140	11.846119
19.317370	1071.459032	11.851123
19.580305	1085.802353	11.856128
19.890284	1084.095544	11.861133
19.495012	1074.633662	11.866138
19.657389	1076.883386	11.871143
19.458825	1094.605673	11.876147
20.061047	1066.150812	11.881152
19.813483	1091.843083	11.886157
19.585008	1065.294820	11.891162
19.793782	1085.609339	11.896167
19.751524	1053.049908	11.901171
20.024611	1107.240343	11.906176
20.286502	1077.757929	11.911181
20.119030	1119.552650	11.916186
20.590794	1089.945272	11.921191
20.116543	1086.009109	11.926195
20.458959	1098.975678	11.931200
20.115385	1090.953210	11.936205
20.114067	1108.044801	11.941210
20.567755	1102.145524	11.946215
20.303630	1097.701173	11.951219
20.554707	1114.058643	11.956224
20.526783	1099.053403	11.961229
20.387183	1119.480305	11.966234
21.074543	1088.444489	11.971239
20.541496	1107.317720	11.976243
20.643574	1113.795499	11.981248
20.749226	1098.902999	11.986253
20.594267	1116.828098	11.991258
20.797918	1095.817039	11.996263
20.430074	1106.157678	12.001267
20.545418	1115.853543	12.006272
20.806715	1104.454466	12.011277
20.837532	1137.902181	12.016282
20.949917	1122.626952	12.021287
21.113380	1133.053183	12.026291
21.262601	1125.784747	12.031296
21.230632	1114.452937	12.036301
21.330350	1107.324872	12.041306
21.319331	1096.160049	12.046311
21.285853	1098.160311	12.051315
21.296361	1097.333911	12.056320
21.541166	1096.198902	12.061325
21.257050	1106.084631	12.066330
21.431901	1094.347682	12.071335
20.885422	1078.341783	12.076339
21.209748	1068.402427	12.081344
21.168216	1071.559896	12.086349
20.785355	1070.286873	12.091354
21.050451	1061.724211	12.096359
20.881276	1082.780262	12.101363
20.775327	1069.402326	12.106368
21.024687	1068.727071	12.111373
20.960988	1071.107470	12.116378
20.969180	1076.244004	12.121383
20.922171	1068.063859	12.126387
21.043018	1078.012715	12.131392
21.287519	1068.746846	12.136397
21.306103	1066.728541	12.141402
21.159862	1081.263277	12.146407
21.116107	1070.606752	12.151411
21.163740	1074.894888	12.156416
21.078718	1087.491219	12.161421
21.117307	1080.935899	12.166426
21.198899	1063.226053	12.171431
20.985609	1083.620503	12.176435
21.132053	1079.333027	12.181440
21.183513	1061.867690	12.186445
20.900529	1084.768038	12.191450
21.447852	1074.457215	12.196455
21.023724	1073.118233	12.201459
20.940789	1091.143779	12.206464
21.284336	1082.762560	12.211469
21.114243	1067.161851	12.216474
21.287966	1069.406610	12.221479
21.000034	1064.212269	12.226483
20.910037	1035.256004	12.231488
20.775436	1057.926060	12.236493
20.997798	1047.838975	12.241498
21.403399	1026.437833	12.246503
21.285474	1061.886625	12.251507
21.346554	1029.845359	12.256512
21.162954	1039.620393	12.261517
20.849600	1055.761888	12.266522
21.027366	1048.198773	12.271527
20.863886	1056.942420	12.276531
20.945587	1041.522357	12.281536
21.130496	1061.181472	12.286541
20.685439	1057.190198	12.291546
21.031724	1043.432646	12.296551
20.862389	1046.320329	12.301555
20.895551	1052.897384	12.306560
21.112783	1045.673334	12.311565
21.037089	1042.909966	12.316570
20.751759	1058.320008	12.321575
20.723188	1049.203362	12.326579
20.675104	1050.016905	12.331584
21.016760	1037.135320	12.336589
20.593395	1069.007377	12.341594
20.886983	1063.909524	12.346599
20.724692	1072.080548	12.351603
20.921106	1087.808030	12.356608
21.107922	1071.440750	12.361613
20.853400	1091.717206	12.366618
21.134522	1087.100737	12.371623
20.939267	1082.624904	12.376627
21.036971	1089.593811	12.381632
21.067145	1087.196756	12.386637
20.820205	1084.940095	12.391642
21.187640	1087.002570	12.396647
21.032415	1097.965316	12.401651
21.446753	1084.190564	12.406656
21.175911	1073.966078	12.411661
20.824286	1067.094525	12.416666
21.130479	1069.900061	12.421671
20.916862	1052.745100	12.426675
21.090240	1059.194136	12.431680
21.073740	1066.151284	12.436685
20.543853	1060.601290	12.441690
21.157934	1059.593470	12.446695
21.161187	1090.623234	12.451699
21.457003	1058.834630	12.456704
21.375823	1054.564543	12.461709
20.980812	1075.382209	12.466714
20.885512	1061.824383	12.471719
21.195155	1063.085505	12.476723
21.082292	1052.820067	12.481728
21.278882	1059.689608	12.486733
20.911098	1066.254922	12.491738
21.086248	1066.337414	12.496743
21.191661	1065.308219	12.501747
21.012189	1060.236932	12.506752
21.323091	1054.680575	12.511757
21.050992	1074.587643	12.516762
21.299408	1053.252533	12.521767
20.991835	1067.999071	12.526771
21.150978	1064.106974	12.531776
20.795717	1049.243881	12.536781
20.857264	1074.177180	12.541786
21.064198	1058.011714	12.546791
21.428773	1077.907130	12.551795
21.160137	1045.931032	12.556800
20.969939	1042.383245	12.561805
21.027495	1054.955231	12.566810
21.450214	1029.708258	12.571815
20.991277	1041.837478	12.576819
21.117282	1041.517794	12.581824
21.088986	1025.847204	12.586829
21.061300	1052.209245	12.591834
21.088763	1039.193264	12.596839
21.124378	1031.007847	12.601843
21.069034	1040.366604	12.606848
21.322410	1032.379848	12.611853
21.018804	1047.251890	12.616858
21.055604	1029.907203	12.621863
21.080034	1046.032660	12.626867
21.089606	1044.170339	12.631872
21.189041	1035.015939	12.636877
20.861410	1038.427192	12.641882
21.050821	1037.764653	12.646887
21.071215	1048.959553	12.651891
21.153616	1039.840983	12.656896
21.151134	1040.287702	12.661901
20.851223	1037.288856	12.666906
20.987104	1031.823502	12.671911
21.156296	1040.931979	12.676915
21.096981	1032.988786	12.681920
20.911920	1020.430925	12.686925
20.654163	1011.246776	12.691930
20.700353	1032.446603	12.696935
21.258449	1046.312295	12.701939
21.398890	1037.619715	12.706944
21.156946	1029.019668	12.711949
20.892552	1024.980664	12.716954
21.046229	1007.278313	12.721959
20.840267	1017.798076	12.726963
20.752916	1004.469274	12.731968
21.121631	1032.818121	12.736973
20.790199	1035.851505	12.741978
21.108127	1029.467701	12.746983
20.921926	1030.910408	12.751987
21.043940	1042.773503	12.756992
20.949111	1042.001755	12.761997
20.571547	1051.115440	12.767002
20.902998	1056.149945	12.772007
21.074265	1057.206052	12.777011
20.971407	1055.099883	12.782016
21.324628	1057.833260	12.787021
20.969331	1051.616747	12.792026
21.070988	1044.004271	12.797031
21.000259	1048.445320	12.802035
21.018606	1052.924204	12.807040
21.072022	1041.085238	12.812045
20.882895	1045.734407	12.817050
21.200356	1046.194753	12.822055
20.893653	1037.532489	12.827059
20.828888	1021.891375	12.832064
20.713797	1051.820280	12.837069
20.894766	1052.903225	12.842074
20.977287	1048.512411	12.847079
20.985235	1058.928700	12.852083
20.927660	1052.030756	12.857088
20.937691	1053.153580	12.862093
21.109531	1054.569147	12.867098
21.152529	1052.379790	12.872103
20.959563	1056.707871	12.877107
21.105276	1058.436692	12.882112
21.297191	1057.663365	12.887117
21.086122	1045.237365	12.892122
20.999982	1022.709848	12.897127
20.891742	1034.895093	12.902131
20.660101	1022.958102	12.907136
21.162068	1039.638178	12.912141
20.692918	1058.652545	12.917146
20.984007	1056.116108	12.922151
21.163961	1058.736769	12.927155
21.196130	1057.000154	12.932160
21.138283	1044.377827	12.937165
20.902128	1045.415334	12.942170
21.027492	1032.566674	12.947175
20.704338	1035.330652	12.952179
20.997582	1051.619825	12.957184
21.426557	1052.485016	12.962189
21.237648	1038.393353	12.967194
21.079212	1032.131258	12.972199
20.726468	1022.047606	12.977203
20.840876	1028.252141	12.982208
21.181544	1031.596227	12.987213
20.786229	1036.921686	12.992218
21.141178	1023.536514	12.997223
20.929015	1032.406185	13.002227
20.782509	1031.387209	13.007232
20.972244	1026.551942	13.012237
20.678408	1042.576767	13.017242
21.233923	1046.851700	13.022247
21.331365	1038.263751	13.027251
21.024761	1033.132324	13.032256
20.904467	1029.216995	13.037261
21.133012	1036.761105	13.042266
21.089807	1025.271882	13.047271
20.689386	1032.197205	13.052275
21.038341	1025.439442	13.057280
21.375394	1037.943181	13.062285
20.989252	1033.051525	13.067290
21.093294	1032.870964	13.072295
20.830091	1034.392185	13.077299
20.828565	1039.527102	13.082304
21.029105	1036.729139	13.087309
21.006761	1035.360773	13.092314
21.246566	1036.890078	13.097319
20.910996	1036.374350	13.102323
21.084075	1037.138425	13.107328
21.144061	1027.619733	13.112333
20.797887	1044.398817	13.117338
21.046671	1034.777466	13.122343
21.260754	1036.006518	13.127347
21.243806	1032.598260	13.132352
21.280428	1042.524255	13.137357
21.020775	1041.119619	13.142362
21.310363	1028.585397	13.147367
20.873628	1048.802544	13.152371
21.028218	1051.808878	13.157376
21.122334	1035.986287	13.162381
20.896821	1046.673195	13.167386
21.443937	1041.585378	13.172391
21.372448	1043.495499	13.177395
20.768670	1028.397671	13.182400
20.998121	1034.568089	13.187405
21.010482	1040.752635	13.192410
21.510153	1025.322696	13.197415
20.982477	1022.555725	13.202419
20.663704	1018.681516	13.207424
21.097474	1000.008817	13.212429
20.796930	1018.833812	13.217434
20.838958	1014.432121	13.222439
20.965339	1025.813528	13.227443
20.844457	1041.198900	13.232448
20.733012	1038.602087	13.237453
20.913326	1049.268425	13.242458
20.991646	1034.061800	13.247463
21.092927	1044.201414	13.252467
20.954118	1041.337724	13.257472
21.252347	1040.255700	13.262477
21.013854	1042.383272	13.267482
21.200313	1035.148365	13.272487
21.104985	1033.905181	13.277491
20.971606	1016.679117	13.282496
21.148185	1017.049967	13.287501
20.549268	1017.907208	13.292506
20.912104	1023.253668	13.297511
21.134357	1045.239152	13.302515
21.216760	1037.345895	13.307520
21.221154	1021.238005	13.312525
20.578335	1017.431250	13.317530
20.979019	1024.340763	13.322535
21.033327	1039.378066	13.327539
20.898210	1032.148719	13.332544
21.261391	1057.838139	13.337549
20.937654	1050.438590	13.342554
21.247844	1014.052478	13.347559
21.073437	1020.943326	13.352563
20.883806	1016.537580	13.357568
21.077775	1031.060584	13.362573
21.157366	1009.017594	13.367578
21.087844	1006.721610	13.372583
20.968968	1015.384000	13.377587
20.970924	1000.514447	13.382592
21.188596	998.760868	13.387597
20.913859	1018.983676	13.392602
21.091204	1010.830859	13.397607
21.033878	1018.283358	13.402611
20.718741	1019.945327	13.407616
20.891898	1016.910458	13.412621
20.939577	1012.536251	13.417626
21.113592	1013.110940	13.422631
20.781709	1019.282571	13.427635
20.520896	1019.638026	13.432640
21.064191	1026.471178	13.437645
21.076642	1027.610961	13.442650
21.103982	1024.599347	13.447655
20.886822	1015.268370	13.452659
21.078082	1015.485489	13.457664
21.101045	1012.969746	13.462669
21.110199	1021.558103	13.467674
21.168315	1013.645078	13.472679
21.199916	1016.450244	13.477683
20.889646	1015.648203	13.482688
20.895846	1017.667356	13.487693
20.935235	1023.399723	13.492698
20.706538	1018.049292	13.497703
20.954021	1020.217623	13.502707
20.680914	1017.107272	13.507712
20.934707	1023.215456	13.512717
21.045142	1044.031310	13.517722
21.184265	1041.017634	13.522727
21.252357	1036.397310	13.527731
21.176506	1032.643628	13.532736
20.963939	1023.717196	13.537741
20.757470	1031.322800	13.542746
20.773791	1019.234299	13.547751
21.071083	1023.253939	13.552755
20.874464	1033.117779	13.557760
21.281448	1025.574888	13.562765
20.998239	1031.633104	13.567770
20.705258	1018.136810	13.572775
21.197170	1031.642455	13.577779
20.778194	1038.454044	13.582784
21.305492	1020.436617	13.587789
20.746424	1024.733192	13.592794
21.239032	1031.049298	13.597799
21.420981	1031.875037	13.602803
21.076237	1031.759747	13.607808
21.225469	1034.292262	13.612813
21.160548	1033.615094	13.617818
21.389841	1033.889226	13.622823
21.107585	1031.141459	13.627827
21.097019	1029.108884	13.632832
21.440219	1029.844249	13.637837
20.869423	1039.638460	13.642842
21.221416	1029.505481	13.647847
21.300248	1029.477177	13.652851
21.059849	1017.308195	13.657856
20.679900	1006.716377	13.662861
20.809552	1003.324169	13.667866
21.028183	1016.070706	13.672871
20.874829	1020.518617	13.677875
21.017092	1032.383204	13.682880
21.350985	1027.584870	13.687885
20.646226	1014.532729	13.692890
20.850754	1025.329231	13.697895
20.646610	1039.231331	13.702899
20.971058	1035.241913	13.707904
21.248298	1036.506623	13.712909
21.159369	1043.976791	13.717914
20.868272	1022.715160	13.722919
21.026427	1046.092298	13.727923
20.716564	1038.537575	13.732928
20.936535	1045.572117	13.737933
20.715955	1047.558058	13.742938
21.078254	1037.764057	13.747943
20.870158	1031.880471	13.752947
20.771420	1035.805581	13.757952
21.083646	1046.651154	13.762957
20.643438	1042.678034	13.767962
20.870277	1040.533475	13.772967
20.675512	1027.953501	13.777971
20.645637	1058.857592	13.782976
21.019319	1021.997702	13.787981
20.831030	1049.922904	13.792986
20.893498	1046.460976	13.797991
20.947734	1044.425948	13.802995
20.610645	1041.303719	13.808000
21.181861	1056.152938	13.813005
20.887656	1067.826967	13.818010
21.126567	1062.121237	13.823015
20.968924	1062.020260	13.828019
20.671228	1064.258204	13.833024
21.062946	1061.436053	13.838029
21.291530	1078.740105	13.843034
20.911012	1056.735734	13.848039
20.744931	1058.375511	13.853043
21.095288	1067.902972	13.858048
21.118019	1069.421171	13.863053
20.506817	1064.346200	13.868058
20.986781	1078.771595	13.873063
21.209151	1079.718627	13.878067
20.949583	1070.821739	13.883072
21.015313	1077.144448	13.888077
21.098446	1084.099906	13.893082
21.170503	1074.699108	13.898087
20.942710	1064.295872	13.903091
20.751217	1061.484736	13.908096
21.178873	1065.575060	13.913101
20.915973	1075.227146	13.918106
20.936780	1077.204553	13.923111
21.248831	1079.726877	13.928115
20.872435	1060.068393	13.933120
21.135676	1053.087741	13.938125
21.054310	1061.373586	13.943130
21.147026	1048.899132	13.948135
20.804412	1049.239248	13.953139
20.608230	1046.168662	13.958144
20.992218	1050.147673	13.963149
20.872870	1064.435249	13.968154
21.340425	1073.119261	13.973159
21.378604	1065.958453	13.978163
20.695578	1060.478616	13.983168
20.959523	1048.749571	13.988173
20.870505	1050.219358	13.993178
21.088353	1061.698170	13.998183
21.227060	1060.542238	14.003187
21.326223	1059.163951	14.008192
21.158213	1053.078793	14.013210
20.916639	1049.774832	14.018227
20.666650	1045.756520	14.023245
21.285710	1038.508746	14.028263
20.827151	1053.035800	14.033280
21.127355	1046.589178	14.038298
21.033057	1047.831161	14.043315
21.149994	1048.525098	14.048333
20.822548	1049.242722	14.053351
20.851366	1058.584664	14.058368
21.142026	1070.271026	14.063386
21.003331	1080.023502	14.068403
21.503072	1080.958393	14.073421
21.428095	1071.288835	14.078439
21.173435	1089.036280	14.083456
21.652248	1081.283913	14.088474
21.394509	1073.092199	14.093491
21.042751	1054.334210	14.098509
21.181830	1049.634098	14.103527
21.130890	1073.321543	14.108544
21.617524	1064.737415	14.113562
21.213505	1068.850683	14.118579
21.155197	1085.339900	14.123597
21.374774	1084.760674	14.128615
21.135377	1086.727342	14.133632
21.318072	1089.391148	14.138650
21.124399	1090.631682	14.143667
21.273634	1084.009356	14.148685
21.487935	1092.650084	14.153703
21.246131	1088.468440	14.158720
21.368881	1082.803552	14.163738
20.896929	1082.120698	14.168755
21.001609	1089.144604	14.173773
21.504060	1110.456764	14.178791
21.961569	1116.623772	14.183808
21.964688	1119.611942	14.188826
21.700624	1117.329259	14.193843
21.521849	1111.909071	14.198861
21.699134	1116.650054	14.203879
21.451732	1124.623575	14.208896
22.067036	1114.504133	14.213914
21.738448	1124.293217	14.218931
21.584812	1126.077905	14.223949
21.575365	1122.397144	14.228967
21.639810	1126.726709	14.233984
21.789956	1117.500969	14.239002
21.895969	1131.074499	14.244019
21.943711	1127.659884	14.249037
21.737156	1125.157251	14.254055
21.863803	1125.829194	14.259072
22.042198	1119.096813	14.264090
21.942527	1119.910241	14.269107
22.094701	1123.525844	14.274125
21.940821	1113.437851	14.279143
21.930291	1124.863995	14.284160
21.788091	1121.563043	14.289178
21.796414	1126.458388	14.294195
21.859547	1124.206885	14.299213
22.303168	1128.159809	14.304231
21.989958	1134.234253	14.309248
22.251176	1126.876776	14.314266
21.954206	1123.035815	14.319283
21.978684	1120.593858	14.324301
21.901170	1123.336923	14.329319
22.174842	1120.367602	14.334336
22.382801	1122.704927	14.339354
22.276615	1121.147366	14.344371
21.753660	1114.495389	14.349389
22.038772	1126.022239	14.354407
21.840684	1136.397680	14.359424
22.036557	1126.442651	14.364442
22.141410	1127.083465	14.369459
22.060913	1127.000392	14.374477
22.238393	1127.775908	14.379495
21.928889	1146.598639	14.384512
22.189074	1150.599701	14.389530
22.021931	1142.244066	14.394547
22.129237	1146.513320	14.399565
22.341913	1141.703917	14.404583
22.361074	1143.643511	14.409600
22.557986	1140.684856	14.414618
22.635647	1139.679968	14.419635
22.690268	1147.879026	14.424653
22.566839	1143.066602	14.429671
22.811528	1142.392137	14.434688
22.942297	1129.474586	14.439706
23.145236	1129.626294	14.444723
22.993844	1136.577812	14.449741
22.812928	1120.933698	14.454759
22.392431	1121.851776	14.459776
22.723343	1108.056069	14.464794
22.594955	1119.327980	14.469811
22.410119	1127.985200	14.474829
22.683953	1133.343121	14.479847
22.485626	1137.958409	14.484864
22.565509	1144.605640	14.489882
22.773844	1139.029322	14.494899
22.673442	1147.069069	14.499917
22.949234	1134.771726	14.504935
22.802201	1138.790544	14.509952
22.951823	1135.257436	14.514970
23.150928	1137.545841	14.519987
23.011327	1146.217879	14.525005
23.267278	1124.809951	14.530023
23.068629	1121.343404	14.535040
22.843747	1109.880958	14.540058
22.909090	1120.195496	14.545075
23.112547	1117.114684	14.550093
23.126385	1113.653573	14.555111
22.669565	1115.743008	14.560128
22.907315	1124.357994	14.565146
23.092965	1126.222270	14.570163
22.730788	1135.485057	14.575181
23.113850	1127.143919	14.580199
23.158361	1134.745284	14.585216
23.230380	1132.497081	14.590234
23.322697	1142.340163	14.595251
23.141258	1132.383963	14.600269
23.284725	1135.728835	14.605287
23.014300	1138.183359	14.610304
23.012735	1133.578009	14.615322
22.827464	1126.980702	14.620339
22.932246	1128.953827	14.625357
23.575586	1125.332539	14.630375
23.384034	1124.578220	14.635392
23.427341	1134.004414	14.640410
23.322225	1128.375851	14.645427
23.397835	1131.704805	14.650445
23.751340	1128.975997	14.655463
23.505446	1134.657475	14.660480
23.537888	1123.820914	14.665498
23.717229	1125.451825	14.670515
23.355442	1130.448671	14.675533
23.507238	1122.399241	14.680551
23.392494	1127.685434	14.685568
23.281242	1127.682768	14.690586
23.427907	1129.853699	14.695603
23.407822	1132.497947	14.700621
23.454893	1138.670654	14.705639
23.343380	1139.061271	14.710656
23.117868	1124.880831	14.715674
23.554165	1124.023229	14.720691
23.246735	1137.249017	14.725709
23.642011	1145.904956	14.730727
23.735098	1155.806124	14.735744
23.775503	1145.146021	14.740762
23.910051	1173.024310	14.745779
23.758882	1167.393640	14.750797
24.191339	1156.442920	14.755815
23.852443	1148.789477	14.760832
23.845840	1138.350800	14.765850
23.829949	1137.088710	14.770867
23.536945	1139.476052	14.775885
23.973659	1152.677546	14.780903
23.982888	1179.460602	14.785920
23.968539	1168.516643	14.790938
23.799886	1163.670527	14.795955
23.676089	1166.759170	14.800973
23.996377	1162.944014	14.805991
23.874310	1175.654226	14.811008
24.113374	1166.367084	14.816026
24.259689	1165.398433	14.821043
24.259623	1180.557177	14.826061
24.252881	1167.881740	14.831079
24.208750	1173.905419	14.836096
24.344423	1168.251021	14.841114
24.418773	1163.696472	14.846131
23.960373	1160.826601	14.851149
24.210097	1154.976272	14.856167
24.084040	1161.488049	14.861184
24.182529	1174.222855	14.866202
24.145503	1160.913628	14.871219
24.044235	1167.816269	14.876237
23.824100	1178.539737	14.881255
23.844614	1183.327767	14.886272
24.056010	1179.237403	14.891290
24.406026	1176.899239	14.896307
24.003124	1179.307261	14.901325
24.272261	1167.303524	14.906343
24.086867	1184.148165	14.911360
24.499114	1191.577654	14.916378
24.659764	1184.805603	14.921395
24.813557	1187.197194	14.926413
24.689827	1171.820747	14.931431
24.309222	1183.290232	14.936448
24.333166	1173.087322	14.941466
24.363583	1184.906516	14.946483
24.225849	1200.541826	14.951501
24.591676	1199.958146	14.956519
24.134323	1211.414725	14.961536
24.360167	1207.469908	14.966554
24.894564	1209.780350	14.971571
24.813298	1207.188509	14.976589
24.991640	1196.869725	14.981607
24.780243	1207.816755	14.986624
24.970547	1194.063841	14.991642
25.225416	1188.989726	14.996659
25.105184	1202.589969	15.001677
25.208971	1188.935799	15.006695
25.154399	1192.416087	15.011712
25.026273	1182.474943	15.016730
25.194336	1171.816483	15.021747
24.787279	1158.481335	15.026765
24.839801	1162.515522	15.031783
25.088988	1177.068240	15.036800
24.901259	1154.603213	15.041818
25.164497	1180.919486	15.046835
24.855401	1150.146527	15.051853
25.001163	1157.362108	15.056871
24.967563	1164.568548	15.061888
25.211789	1169.498639	15.066906
25.116758	1169.399008	15.071923
25.395519	1193.008895	15.076941
25.044099	1152.910251	15.081959
25.040466	1178.369347	15.086976
25.092571	1187.932593	15.091994
25.507722	1178.725894	15.097011
25.087025	1183.606316	15.102029
25.466782	1207.215848	15.107047
25.508386	1178.825001	15.112064
25.133056	1195.764441	15.117082
24.986016	1174.082525	15.122099
25.168199	1199.567075	15.127117
25.314412	1195.082849	15.132135
25.622414	1195.198926	15.137152
25.249917	1207.845291	15.142170
25.543159	1191.150235	15.147187
25.231257	1187.887345	15.152205
25.584714	1186.462526	15.157223
25.459897	1195.991077	15.162240
25.238070	1201.929855	15.167258
25.349666	1189.908756	15.172275
24.867733	1189.638033	15.177293
25.082382	1183.069721	15.182311
25.206221	1201.466345	15.187328
25.667728	1222.407688	15.192346
25.718969	1208.796485	15.197363
25.744834	1225.064804	15.202381
25.714477	1226.133015	15.207399
25.917992	1227.867044	15.212416
25.811507	1212.067820	15.217434
26.009259	1216.412329	15.222451
25.875424	1211.447390	15.227469
26.399981	1199.295928	15.232487
26.121312	1198.316408	15.237504
25.695876	1188.339311	15.242522
26.006089	1188.780640	15.247539
25.529768	1200.812797	15.252557
25.953182	1187.658191	15.257575
25.898378	1173.126445	15.262592
25.601619	1199.558807	15.267610
26.007877	1209.948020	15.272627
26.174511	1225.940640	15.277645
26.345154	1208.926927	15.282663
26.113890	1196.107955	15.287680
25.936234	1198.775774	15.292698
26.194979	1184.159403	15.297715
26.161208	1201.418740	15.302733
25.834585	1206.992003	15.307751
25.992152	1201.219272	15.312768
26.117382	1202.821072	15.317786
26.337377	1233.451133	15.322803
26.453189	1218.715956	15.327821
26.441054	1209.314700	15.332839
26.269371	1231.090050	15.337856
26.140645	1228.177022	15.342874
26.664191	1216.334010	15.347891
26.366401	1219.842084	15.352909
26.636036	1223.004839	15.357927
26.665884	1217.323256	15.362944
26.629889	1206.121607	15.367962
26.386946	1190.186874	15.372979
26.289273	1192.863956	15.377997
26.158501	1195.500702	15.383015
26.544632	1204.559243	15.388032
26.707915	1219.507937	15.393050
26.939484	1220.361345	15.398067
26.668967	1204.580426	15.403085
26.353434	1198.246099	15.408103
26.664086	1191.901563	15.413120
26.624624	1216.559507	15.418138
26.692834	1211.515154	15.423155
26.751745	1214.439391	15.428173
26.717841	1219.657669	15.433191
27.041101	1222.369865	15.438208
26.685439	1209.503084	15.443226
26.523266	1207.075152	15.448243
26.634742	1211.153430	15.453261
26.722524	1211.955841	15.458279
26.830977	1213.269317	15.463296
26.827148	1223.112060	15.468314
26.687541	1212.200629	15.473331
26.522174	1212.164124	15.478349
26.518136	1212.529736	15.483367
26.753043	1208.323932	15.488384
26.894576	1223.175429	15.493402
27.144925	1213.938365	15.498419
27.002406	1212.334681	15.503437
26.509160	1221.849653	15.508455
27.124959	1231.827949	15.513472
27.031177	1239.627598	15.518490
27.433935	1249.207316	15.523507
27.359261	1247.641569	15.528525
26.875249	1249.285488	15.533543
27.231075	1244.277047	15.538560
27.124671	1256.511365	15.543578
27.335454	1234.994079	15.548595
27.247290	1248.971484	15.553613
27.067605	1255.937009	15.558631
27.405969	1240.661389	15.563648
27.246524	1243.892583	15.568666
27.404919	1240.540515	15.573683
27.325722	1236.035600	15.578701
27.151032	1246.449858	15.583719
27.182593	1239.396359	15.588736
27.096643	1236.553583	15.593754
27.235821	1248.852543	15.598771
27.739113	1261.584210	15.603789
27.576464	1259.875195	15.608807
27.909484	1253.921882	15.613824
27.634706	1258.060205	15.618842
27.848707	1235.342223	15.623859
27.667003	1230.674340	15.628877
27.552338	1227.266729	15.633895
28.073446	1227.696445	15.638912
27.694043	1237.330119	15.643930
27.848278	1232.937407	15.648947
27.954124	1225.960153	15.653965
27.424816	1235.020004	15.658983
27.829164	1231.172548	15.664000
27.713534	1226.778836	15.669018
27.869456	1241.865576	15.674035
27.889936	1255.275118	15.679053
28.118787	1249.233032	15.684071
28.114501	1229.162589	15.689088
27.861972	1237.539670	15.694106
28.111440	1229.639765	15.699123
28.430251	1228.078901	15.704141
27.892410	1232.926115	15.709159
28.017167	1224.228157	15.714176
27.749793	1240.407986	15.719194
28.083102	1246.261390	15.724211
28.134909	1247.708169	15.729229
28.064826	1252.652239	15.734247
28.588369	1246.946960	15.739264
28.148852	1247.275066	15.744282
28.268395	1246.477415	15.749299
28.549183	1257.232729	15.754317
28.023336	1261.044593	15.759335
28.237109	1257.035622	15.764352
28.284307	1267.914713	15.769370
28.358536	1267.218668	15.774387
28.667183	1267.592611	15.779405
28.514832	1263.745849	15.784423
28.770466	1255.074189	15.789440
28.517753	1242.917674	15.794458
28.661373	1235.022065	15.799475
28.435264	1222.954128	15.804493
28.422941	1243.219193	15.809511
28.695278	1245.966256	15.814528
28.604989	1258.265644	15.819546
28.552759	1255.747811	15.824563
28.682384	1264.159909	15.829581
28.387926	1267.508593	15.834599
28.330976	1250.104853	15.839616
28.530064	1267.122642	15.844634
28.451673	1277.309211	15.849651
28.636543	1268.125027	15.854669
28.399867	1273.293871	15.859687
28.593673	1279.951308	15.864704
28.985604	1266.767046	15.869722
28.784396	1283.077937	15.874739
28.736277	1268.209985	15.879757
28.644636	1273.988034	15.884775
29.048768	1269.250297	15.889792
28.969683	1284.162211	15.894810
28.947960	1302.752847	15.899827
29.403054	1274.667875	15.904845
29.058815	1300.798904	15.909863
29.291677	1291.128864	15.914880
28.951345	1264.819258	15.919898
28.815419	1302.193750	15.924915
29.370436	1275.738178	15.929933
29.020513	1305.583926	15.934951
29.302811	1289.568458	15.939968
29.228160	1300.209038	15.944986
29.265849	1292.441975	15.950003
29.650577	1279.155820	15.955021
29.300908	1296.373633	15.960039
29.562219	1282.775260	15.965056
29.265528	1279.711264	15.970074
29.283177	1282.719171	15.975091
29.497208	1286.892010	15.980109
29.511734	1299.530209	15.985127
29.514049	1291.493517	15.990144
29.760065	1268.017706	15.995162
29.302487	1277.339841	16.000179
29.571995	1280.703969	16.005197
29.595647	1289.308371	16.010215
29.793653	1285.931886	16.015232
29.501457	1272.383264	16.020250
29.544721	1294.120494	16.025267
29.531284	1278.121532	16.030285
29.471846	1301.215331	16.035303
29.640305	1293.636617	16.040320
29.938707	1296.071228	16.045338
29.718272	1287.646932	16.050355
29.910096	1286.292713	16.055373
29.819576	1300.164367	16.060391
29.735250	1305.876770	16.065408
30.080776	1285.880228	16.070426
29.970081	1288.697040	16.075443
30.031378	1285.561004	16.080461
29.574623	1289.961947	16.085479
29.707566	1293.349433	16.090496
29.829669	1299.692708	16.095514
29.597289	1297.124951	16.100531
30.207439	1282.629396	16.105549
30.027531	1291.151437	16.110567
30.059532	1300.571677	16.115584
30.100194	1289.524474	16.120602
30.376506	1292.376302	16.125619
29.956311	1279.334925	16.130637
30.006326	1310.430335	16.135655
30.351481	1311.811459	16.140672
30.541890	1307.703957	16.145690
30.366642	1331.200869	16.150707
30.540888	1294.044418	16.155725
30.334782	1320.221875	16.160743
30.461962	1282.147260	16.165760
30.415398	1304.098600	16.170778
30.434905	1320.207596	16.175795
30.792194	1298.306636	16.180813
30.360250	1310.408881	16.185831
30.428558	1310.116461	16.190848
30.947254	1305.648297	16.195866
30.603977	1300.933803	16.200883
30.542943	1297.063030	16.205901
30.228493	1308.658910	16.210919
30.744947	1306.363393	16.215936
30.909090	1315.120790	16.220954
30.855559	1330.487987	16.225971
30.983375	1307.365224	16.230989
30.831523	1301.533268	16.236007
30.841504	1295.348323	16.241024
30.964729	1293.873701	16.246042
30.651422	1274.355048	16.251059
30.664066	1306.983774	16.256077
30.988755	1311.218407	16.261095
31.023893	1306.092782	16.266112
31.109310	1309.259769	16.271130
31.029329	1329.199126	16.276147
31.411665	1290.164385	16.281165
30.959461	1296.232750	16.286183
31.042010	1280.484311	16.291200
31.230508	1274.377866	16.296218
30.700867	1282.698499	16.301235
31.159627	1306.607831	16.306253
31.261016	1311.283907	16.311271
31.167501	1306.432052	16.316288
31.440506	1308.177030	16.321306
31.194228	1318.091538	16.326323
31.310506	1316.124104	16.331341
31.353427	1333.486195	16.336359
31.212218	1302.956687	16.341376
31.677021	1326.282298	16.346394
31.282547	1304.869305	16.351411
31.428799	1315.026365	16.356429
31.457062	1306.850248	16.361447
31.341615	1302.174920	16.366464
31.584944	1310.930697	16.371482
30.849849	1314.687859	16.376499
31.388017	1305.203492	16.381517
31.546146	1315.729881	16.386535
31.507074	1301.843566	16.391552
31.563352	1312.433387	16.396570
31.580954	1332.654480	16.401587
31.521403	1311.843995	16.406605
31.877082	1319.321898	16.411623
31.813306	1345.313110	16.416640
31.939071	1315.505468	16.421658
31.553686	1323.167631	16.426675
31.681375	1334.518414	16.431693
31.952025	1342.280444	16.436711
31.742300	1340.884087	16.441728
32.151253	1344.771818	16.446746
32.002538	1342.755411	16.451763
32.033153	1337.138152	16.456781
31.868411	1338.591164	16.461799
31.877292	1341.419589	16.466816
32.104276	1344.335922	16.471834
31.834388	1344.725062	16.476851
31.949151	1335.259441	16.481869
31.954689	1332.134647	16.486887
32.014189	1336.619217	16.491904
32.450285	1341.007546	16.496922
32.149734	1338.883225	16.501939
32.188091	1336.226665	16.506957
32.316645	1343.819454	16.511975
32.431982	1334.709237	16.516992
32.436189	1333.599650	16.522010
32.194831	1340.955714	16.527027
32.430751	1336.455564	16.532045
32.395403	1336.513149	16.537063
32.404224	1361.468798	16.542080
32.784372	1352.687561	16.547098
32.697200	1357.812140	16.552115
32.715767	1347.188405	16.557133
32.497110	1336.061405	16.562151
32.363446	1332.052772	16.567168
32.629594	1351.535845	16.572186
32.938996	1366.695762	16.577203
32.623487	1350.506590	16.582221
32.894402	1366.440263	16.587239
32.972906	1365.392754	16.592256
33.157072	1357.284551	16.597274
32.558293	1336.902943	16.602291
32.969980	1342.773772	16.607309
33.169348	1341.013302	16.612327
32.761039	1329.537464	16.617344
32.964815	1335.789080	16.622362
33.156701	1363.729377	16.627379
33.254931	1346.261448	16.632397
32.938814	1345.682709	16.637415
32.843455	1347.296111	16.642432
33.016515	1354.790575	16.647450
33.079347	1350.553975	16.652467
33.175602	1369.132959	16.657485
33.127963	1365.777545	16.662503
33.391919	1360.426648	16.667520
33.413665	1363.350551	16.672538
33.228333	1365.392001	16.677555
33.305847	1356.050282	16.682573
33.399942	1358.313000	16.687591
33.272217	1363.667414	16.692608
33.383454	1355.874430	16.697626
33.581849	1358.038718	16.702643
33.191308	1355.140680	16.707661
33.431376	1359.050631	16.712679
33.194641	1359.398305	16.717696
33.704436	1357.413721	16.722714
33.473219	1365.315580	16.727731
33.590693	1356.642300	16.732749
33.374156	1354.545475	16.737767
33.186840	1366.939079	16.742784
33.829342	1369.561063	16.747802
33.712579	1382.791270	16.752819
33.920476	1391.371852	16.757837
33.828150	1385.939346	16.762855
34.281971	1375.722788	16.767872
34.472585	1359.072221	16.772890
33.866861	1356.549840	16.777907
34.024150	1345.092320	16.782925
34.004923	1343.984896	16.787943
33.912009	1351.686942	16.792960
34.281541	1345.529573	16.797978
34.204687	1352.159427	16.802995
34.088715	1343.377099	16.808013
34.301994	1348.700716	16.813031
34.447366	1347.953995	16.818048
34.237926	1336.325315	16.823066
34.211439	1347.442728	16.828083
34.256772	1359.928206	16.833101
34.218881	1345.473812	16.838119
33.980922	1345.225519	16.843136
34.080730	1349.853097	16.848154
33.851794	1359.193872	16.853171
33.925570	1348.171230	16.858189
34.108960	1364.501096	16.863207
34.244753	1374.595374	16.868224
34.674314	1374.206012	16.873242
34.184450	1382.226208	16.878259
34.444667	1373.972162	16.883277
34.717011	1377.954047	16.888295
34.416107	1378.805874	16.893312
34.657453	1388.126718	16.898330
34.267534	1386.730781	16.903347
34.380322	1377.812849	16.908365
34.518779	1381.422841	16.913383
34.718464	1407.345404	16.918400
34.564853	1396.826170	16.923418
35.203657	1416.080012	16.928435
35.324632	1409.451035	16.933453
35.406477	1376.408333	16.938471
35.107462	1373.171657	16.943488
35.190545	1367.635678	16.948506
35.195157	1369.587062	16.953523
35.255229	1374.431766	16.958541
35.225507	1367.188209	16.963559
34.936803	1372.815260	16.968576
35.491188	1366.944571	16.973594
34.897768	1367.808445	16.978611
34.933208	1372.021589	16.983629
35.147164	1367.753017	16.988647
34.936250	1379.167276	16.993664
35.153212	1371.568202	16.998682
35.019433	1367.727888	17.003699
35.029794	1376.884221	17.008717
35.343029	1394.816740	17.013735
35.720271	1401.470146	17.018752
36.058061	1390.770298	17.023770
35.410795	1378.945575	17.028787
35.405519	1376.289675	17.033805
35.415717	1372.225054	17.038823
35.564886	1398.783282	17.043840
35.720734	1394.407567	17.048858
35.701128	1382.857110	17.053875
35.484941	1391.242639	17.058893
35.579200	1385.914079	17.063911
35.870888	1402.215705	17.068928
35.940071	1401.825619	17.073946
35.946928	1395.477538	17.078963
35.768536	1393.119799	17.083981
35.868897	1380.994943	17.088999
35.617704	1389.774584	17.094016
35.620951	1398.691398	17.099034
35.963707	1400.055611	17.104051
35.968464	1400.561395	17.109069
35.903495	1402.649719	17.114087
35.856898	1402.610000	17.119104
36.266042	1393.986132	17.124122
36.256509	1391.658090	17.129139
36.167949	1395.208339	17.134157
36.201798	1393.261907	17.139175
35.819854	1400.588513	17.144192
35.520990	1404.468029	17.149210
36.068192	1405.810646	17.154227
35.807099	1408.776522	17.159245
36.127377	1413.592324	17.164263
36.164142	1426.816960	17.169280
36.472683	1426.155895	17.174298
36.510160	1423.609569	17.179315
36.340413	1432.637363	17.184333
36.807110	1416.394148	17.189351
36.504896	1427.793120	17.194368
36.522870	1426.638859	17.199386
36.786249	1425.845001	17.204403
36.634164	1430.149417	17.209421
36.884668	1424.377507	17.214439
36.776347	1417.467351	17.219456
36.833764	1427.560008	17.224474
36.736596	1427.012411	17.229491
36.468217	1434.893493	17.234509
36.621311	1421.226522	17.239527
36.777770	1428.171551	17.244544
36.602568	1420.979483	17.249562
36.602267	1416.905513	17.254579
36.630983	1431.308037	17.259597
37.365895	1433.511036	17.264615
36.868881	1438.881904	17.269632
37.149625	1438.714474	17.274650
37.488572	1449.528295	17.279667
37.187752	1439.224413	17.284685
37.470392	1425.165550	17.289703
37.414817	1415.467500	17.294720
37.179262	1414.015481	17.299738
37.405347	1409.738670	17.304755
37.185917	1416.911953	17.309773
37.270305	1413.074583	17.314791
37.147938	1420.098683	17.319808
37.392888	1432.538231	17.324826
37.630037	1429.864106	17.329843
37.307223	1440.640321	17.334861
37.880604	1447.628975	17.339879
37.723735	1432.246525	17.344896
37.486590	1419.735025	17.349914
37.708612	1411.820524	17.354931
37.840846	1416.295092	17.359949
37.670964	1403.488167	17.364967
37.481379	1415.636787	17.369984
37.174390	1419.577376	17.375002
37.511429	1433.282655	17.380019
37.479549	1448.898203	17.385037
37.881547	1441.313626	17.390055
38.024319	1446.961551	17.395072
37.969502	1454.478254	17.400090
37.961356	1448.824663	17.405107
37.901170	1443.663856	17.410125
38.099529	1444.668865	17.415143
38.024567	1447.203948	17.420160
37.878276	1437.830231	17.425178
38.329074	1437.113444	17.430195
37.919673	1450.527235	17.435213
38.020741	1441.007102	17.440231
38.076956	1432.107597	17.445248
38.148710	1435.169827	17.450266
38.351905	1450.886310	17.455283
38.316256	1466.090353	17.460301
38.503120	1463.699517	17.465319
38.647606	1461.853405	17.470336
38.255162	1459.367775	17.475354
38.531279	1451.523275	17.480371
38.714238	1466.067972	17.485389
38.798158	1460.492500	17.490407
38.608119	1452.514709	17.495424
38.630835	1438.053702	17.500442
38.701413	1440.449171	17.505459
38.279581	1450.659176	17.510477
38.821540	1458.739789	17.515495
38.927265	1461.752563	17.520512
38.497867	1472.405803	17.525530
38.477661	1471.558071	17.530547
38.665064	1468.350761	17.535565
39.019511	1466.705540	17.540583
38.892175	1467.789235	17.545600
38.964322	1462.910906	17.550618
39.014250	1462.314680	17.555635
38.812633	1470.653887	17.560653
39.388120	1468.339494	17.565671
39.299896	1484.846521	17.570688
39.055578	1467.283642	17.575706
39.255877	1461.678597	17.580723
38.919935	1470.301919	17.585741
39.108427	1460.549183	17.590759
38.918362	1461.178847	17.595776
38.998077	1476.666518	17.600794
39.242031	1486.948114	17.605811
39.390653	1497.200877	17.610829
39.796649	1489.689568	17.615847
39.682731	1497.377738	17.620864
39.778136	1493.990042	17.625882
39.900379	1484.221115	17.630899
39.594936	1477.240124	17.635917
39.758584	1457.381676	17.640935
39.521802	1456.559048	17.645952
39.500493	1465.951720	17.650970
39.944743	1469.042637	17.655987
39.513956	1475.673940	17.661005
39.854260	1479.544343	17.666023
39.913920	1491.137330	17.671040
39.834355	1489.625819	17.676058
40.065259	1489.074660	17.681075
39.836788	1484.228538	17.686093
39.938952	1488.965896	17.691111
39.983451	1494.146601	17.696128
40.303263	1497.235348	17.701146
40.397938	1482.710911	17.706163
39.836800	1497.070724	17.711181
40.170647	1489.912264	17.716199
40.067065	1497.855185	17.721216
39.868358	1496.884912	17.726234
39.911946	1485.082051	17.731251
39.872148	1494.328254	17.736269
40.150597	1490.301041	17.741287
40.156470	1489.117245	17.746304
40.326669	1496.063262	17.751322
40.395549	1496.137257	17.756339
40.391793	1508.317665	17.761357
40.630309	1492.560637	17.766375
40.825734	1505.363645	17.771392
40.819920	1509.643183	17.776410
40.993562	1499.131455	17.781427
40.896393	1504.702841	17.786445
40.942800	1494.749376	17.791463
40.595985	1485.560190	17.796480
40.430969	1489.861967	17.801498
40.818913	1486.443347	17.806515
40.398298	1492.351027	17.811533
40.988206	1498.806969	17.816551
41.200458	1504.480015	17.821568
40.576108	1510.541316	17.826586
40.990551	1496.359118	17.831603
41.008921	1501.951401	17.836621
40.751129	1496.227496	17.841639
41.062205	1494.189646	17.846656
41.108720	1491.420073	17.851674
41.400504	1486.781982	17.856691
41.148913	1492.475518	17.861709
41.286960	1489.370454	17.866727
41.549552	1495.905339	17.871744
41.358619	1503.967586	17.876762
41.442085	1497.857350	17.881779
41.368488	1495.872985	17.886797
41.230263	1506.105437	17.891815
41.471781	1520.084006	17.896832
41.711707	1523.007750	17.901850
41.948342	1513.775831	17.906867
41.789879	1510.595358	17.911885
41.806597	1497.876564	17.916903
41.891858	1478.029017	17.921920
41.509412	1492.212464	17.926938
41.683042	1489.067120	17.931955
41.917255	1498.197267	17.936973
41.993849	1509.847343	17.941991
42.057260	1494.945640	17.947008
41.833817	1492.271030	17.952026
41.991372	1482.872420	17.957043
41.928261	1501.728672	17.962061
42.298181	1521.955187	17.967079
42.553732	1514.673923	17.972096
41.923861	1504.603368	17.977114
42.036740	1498.005529	17.982131
42.106397	1512.820025	17.987149
42.146169	1515.369854	17.992167
42.363407	1512.266313	17.997184
42.110300	1523.928085	18.002202
42.507651	1516.059497	18.007219
42.178473	1520.544765	18.012237
41.959839	1517.929158	18.017255
42.493115	1506.131551	18.022272
42.155357	1516.269992	18.027290
42.100044	1509.843688	18.032307
42.363457	1517.586520	18.037325
42.630481	1533.325946	18.042343
42.644520	1547.930700	18.047360
42.566737	1552.286222	18.052378
42.629858	1531.702819	18.057395
43.074070	1548.335785	18.062413
42.522426	1542.171093	18.067431
43.161424	1542.825838	18.072448
42.488620	1540.257492	18.077466
43.104013	1541.170829	18.082483
43.133105	1542.762832	18.087501
42.820669	1546.364553	18.092519
43.071448	1546.316731	18.097536
43.009919	1533.391738	18.102554
43.224940	1532.424690	18.107571
42.978483	1527.886585	18.112589
42.913217	1536.540707	18.117607
43.214090	1551.194099	18.122624
43.355436	1562.684455	18.127642
43.317170	1556.140582	18.132659
43.630885	1566.030440	18.137677
43.759494	1564.985938	18.142695
43.531255	1543.862252	18.147712
43.150418	1551.928071	18.152730
43.588816	1566.353480	18.157747
43.665942	1569.852179	18.162765
43.279802	1573.709478	18.167783
43.798399	1569.467766	18.172800
43.881686	1573.426376	18.177818
43.777478	1567.621319	18.182835
43.908574	1567.707415	18.187853
43.797936	1571.643470	18.192871
44.168437	1562.836905	18.197888
43.692330	1571.997015	18.202906
44.263131	1564.572641	18.207923
44.007932	1562.257011	18.212941
43.947388	1577.224470	18.217959
43.993493	1567.730323	18.222976
44.171432	1560.508605	18.227994
44.106180	1572.813704	18.233011
43.981026	1559.563783	18.238029
44.267011	1560.048316	18.243047
44.185740	1563.565983	18.248064
43.914623	1573.125979	18.253082
44.514505	1563.269811	18.258099
44.252863	1565.817384	18.263117
43.888862	1565.512110	18.268135
44.327050	1575.361674	18.273152
44.410357	1590.310924	18.278170
44.520605	1596.272406	18.283187
44.602924	1599.249616	18.288205
44.629963	1601.504192	18.293223
44.965765	1591.402260	18.298240
44.604670	1597.709473	18.303258
45.076949	1593.866822	18.308275
45.206454	1590.242432	18.313293
44.721353	1595.883587	18.318311
45.058047	1586.879480	18.323328
44.867222	1597.219485	18.328346
44.887630	1594.826860	18.333363
44.988003	1591.263745	18.338381
44.885630	1587.574091	18.343399
44.859116	1579.140718	18.348416
44.813916	1589.223112	18.353434
44.997059	1581.465730	18.358451
45.177823	1587.107651	18.363469
44.914587	1590.844681	18.368487
45.434268	1604.560320	18.373504
45.789888	1602.391084	18.378522
45.501371	1594.230721	18.383539
45.471159	1582.828085	18.388557
45.579766	1590.054528	18.393575
45.728811	1578.863978	18.398592
45.524460	1586.432911	18.403610
45.504608	1578.923407	18.408627
45.563062	1583.779452	18.413645
45.290304	1609.288518	18.418663
45.662884	1614.478290	18.423680
45.810633	1610.149421	18.428698
45.720358	1617.512988	18.433715
45.980255	1606.106538	18.438733
45.811391	1607.657760	18.443751
45.868380	1606.162210	18.448768
45.784345	1610.193133	18.453786
45.743355	1612.672490	18.458803
45.596581	1607.690600	18.463821
45.700616	1623.067584	18.468839
46.040569	1618.925135	18.473856
46.135255	1628.878283	18.478874
46.274739	1641.970331	18.483891
46.058388	1640.782639	18.488909
46.454197	1648.737232	18.493927
46.647483	1636.633523	18.498944
46.518384	1641.601295	18.503962
46.414377	1628.141873	18.508979
46.946407	1632.952293	18.513997
46.609553	1638.030275	18.519015
46.881524	1629.148150	18.524032
46.886744	1631.401491	18.529050
46.951865	1635.951324	18.534067
46.660568	1625.877022	18.539085
46.665636	1632.034617	18.544103
46.763880	1635.374236	18.549120
46.786277	1634.865763	18.554138
47.066583	1639.066675	18.559155
47.013383	1625.762746	18.564173
46.740274	1632.208523	18.569191
47.022446	1628.684045	18.574208
47.029198	1627.393132	18.579226
47.117050	1629.335994	18.584243
46.900137	1622.877211	18.589261
47.026601	1633.657420	18.594279
46.806497	1630.809220	18.599296
46.973142	1621.114916	18.604314
46.998242	1644.673191	18.609331
47.368699	1650.638814	18.614349
47.252371	1674.211827	18.619367
47.578818	1663.601679	18.624384
47.535273	1667.503464	18.629402
47.485037	1663.176267	18.634419
48.002218	1652.535708	18.639437
47.873377	1660.783193	18.644455
47.832788	1652.858535	18.649472
47.754024	1651.350024	18.654490
47.784929	1653.869832	18.659507
48.013268	1647.429690	18.664525
47.627890	1651.337224	18.669543
47.798845	1653.480766	18.674560
48.226460	1647.535804	18.679578
47.745017	1651.290346	18.684595
47.829428	1653.549937	18.689613
47.816228	1659.225966	18.694631
48.335695	1643.899020	18.699648
47.988869	1643.266962	18.704666
47.995836	1646.547209	18.709683
48.146151	1653.027713	18.714701
48.257507	1659.764543	18.719719
48.333786	1659.653316	18.724736
48.676015	1686.355888	18.729754
48.487587	1661.220763	18.734771
48.689202	1694.049098	18.739789
48.629725	1664.540842	18.744807
49.079972	1672.062051	18.749824
48.531480	1648.838964	18.754842
48.620316	1661.536415	18.759859
48.921771	1637.372407	18.764877
48.650913	1639.177424	18.769895
48.483112	1647.684372	18.774912
48.717348	1665.370279	18.779930
48.807751	1669.571599	18.784947
48.745660	1667.288074	18.789965
48.585325	1688.971065	18.794983
48.927153	1668.528635	18.800000
48.939114	1667.916434	18.805018
49.023979	1680.509141	18.810035
49.075849	1663.507547	18.815053
48.698772	1671.973952	18.820071
49.094302	1684.037345	18.825088
49.138802	1699.018065	18.830106
49.264331	1696.526862	18.835123
49.516906	1697.447737	18.840141
48.989224	1683.097860	18.845159
49.202721	1697.924212	18.850176
49.579652	1697.763463	18.855194
49.193378	1700.573181	18.860211
49.667515	1692.714275	18.865229
49.710428	1706.425824	18.870247
49.767603	1696.080394	18.875264
49.884285	1705.770538	18.880282
50.254264	1710.024810	18.885299
50.029735	1686.934039	18.890317
49.915789	1716.690300	18.895335
49.956209	1682.753734	18.900352
50.151782	1683.109546	18.905370
49.917647	1685.592977	18.910387
50.486037	1692.882998	18.915405
50.353153	1703.580352	18.920423
50.081977	1699.741411	18.925440
50.330002	1685.519504	18.930458
50.110131	1695.777694	18.935475
50.650180	1700.704836	18.940493
50.401433	1716.756382	18.945511
50.391956	1716.790965	18.950528
50.615694	1711.207256	18.955546
50.471777	1720.253130	18.960563
50.736394	1717.626483	18.965581
50.794482	1727.937894	18.970599
50.882951	1713.031971	18.975616
50.955155	1701.955828	18.980634
50.308933	1700.679384	18.985651
50.838665	1694.302839	18.990669
50.825242	1712.559983	18.995687
50.670121	1712.869479	19.000704
50.915716	1712.127207	19.005722
50.821169	1714.939166	19.010739
51.070213	1702.848531	19.015757
50.831562	1710.948390	19.020775
51.031597	1714.341006	19.025792
51.197257	1714.718893	19.030810
50.982495	1716.010031	19.035827
51.192805	1707.508927	19.040845
50.948877	1716.256143	19.045863
50.831538	1729.112376	19.050880
51.284950	1729.400328	19.055898
50.833986	1737.159680	19.060915
51.145318	1744.567802	19.065933
51.321192	1736.816215	19.070951
51.242750	1739.713700	19.075968
51.417813	1745.436818	19.080986
51.551645	1765.875933	19.086003
52.354580	1755.752873	19.091021
52.006137	1763.676788	19.096039
52.171258	1768.545770	19.101056
52.141809	1767.004214	19.106074
52.228570	1771.830639	19.111091
51.797330	1760.719910	19.116109
52.150632	1751.068111	19.121127
52.265122	1757.960218	19.126144
52.461271	1764.796833	19.131162
52.624381	1758.020978	19.136179
52.671849	1744.016616	19.141197
52.367103	1726.137442	19.146215
52.344415	1731.495688	19.151232
52.408027	1728.539299	19.156250
52.111024	1727.092327	19.161267
52.159877	1734.254440	19.166285
52.531850	1751.415117	19.171303
52.228759	1760.415615	19.176320
52.613008	1751.630341	19.181338
52.573456	1764.172177	19.186355
52.763733	1749.294025	19.191373
52.568063	1754.712901	19.196391
52.190158	1763.195221	19.201408
52.862904	1769.114257	19.206426
52.628810	1781.325337	19.211443
53.119359	1781.679727	19.216461
53.526316	1775.225200	19.221479
53.047450	1782.392846	19.226496
53.360303	1783.829508	19.231514
53.479340	1789.956410	19.236531
53.427227	1776.225877	19.241549
53.215931	1768.584784	19.246567
53.374451	1784.683138	19.251584
53.646656	1784.037293	19.256602
53.285197	1788.411385	19.261619
53.814815	1784.674373	19.266637
53.486565	1777.915523	19.271655
53.599978	1781.542194	19.276672
53.325927	1786.946841	19.281690
53.348203	1780.501751	19.286707
53.870919	1770.080449	19.291725
53.715510	1780.616284	19.296743
53.747062	1778.484548	19.301760
54.004076	1764.122704	19.306778
53.631841	1783.598059	19.311795
53.818693	1771.462230	19.316813
54.141836	1775.678374	19.321831
54.043291	1767.402670	19.326848
54.000273	1774.175185	19.331866
54.219746	1779.960447	19.336883
54.111651	1775.132781	19.341901
54.171465	1780.381933	19.346919
54.001610	1804.234255	19.351936
54.429668	1808.669632	19.356954
54.324781	1814.899897	19.361971
54.514280	1802.428563	19.366989
54.385484	1809.375224	19.372007
54.447554	1803.859734	19.377024
54.569869	1790.327887	19.382042
54.338721	1804.191776	19.387059
54.830039	1794.819961	19.392077
54.960315	1805.959916	19.397095
54.672476	1800.413714	19.402112
54.990400	1801.520805	19.407130
54.747370	1819.918522	19.412147
54.925054	1822.901020	19.417165
54.971680	1819.969344	19.422183
55.181104	1826.289488	19.427200
55.314751	1821.302129	19.432218
55.244822	1837.012253	19.437235
55.698222	1825.098142	19.442253
55.557518	1830.492549	19.447271
55.683199	1829.004898	19.452288
55.712197	1824.620971	19.457306
55.563908	1832.936150	19.462323
55.645455	1827.299567	19.467341
55.608538	1818.704117	19.472359
55.807013	1820.799251	19.477376
55.767754	1820.651393	19.482394
55.626400	1816.011490	19.487411
55.742322	1829.310388	19.492429
55.987273	1820.986165	19.497447
55.642613	1820.713978	19.502464
55.608270	1821.690059	19.507482
55.835884	1820.043006	19.512499
55.900283	1825.692568	19.517517
55.503287	1823.902880	19.522535
55.866733	1831.957120	19.527552
56.025534	1842.737048	19.532570
56.230384	1848.642648	19.537587
56.343257	1839.623744	19.542605
56.714768	1834.236647	19.547623
56.314812	1839.376672	19.552640
56.642206	1832.263120	19.557658
56.783028	1831.101820	19.562675
56.643470	1833.534013	19.567693
56.781290	1834.471626	19.572711
56.653357	1838.882423	19.577728
56.970598	1827.561038	19.582746
56.365066	1835.609362	19.587763
56.553746	1834.179305	19.592781
56.914665	1833.821334	19.597799
56.635403	1833.640964	19.602816
56.610499	1842.356473	19.607834
56.856621	1842.056135	19.612851
56.971670	1859.128925	19.617869
57.539758	1863.249402	19.622887
57.127605	1858.703009	19.627904
57.636594	1854.409267	19.632922
57.470914	1860.908798	19.637939
57.333266	1862.893946	19.642957
57.473750	1847.551722	19.647975
57.311056	1858.099785	19.652992
57.404791	1851.139894	19.658010
57.454181	1856.266465	19.663027
57.357745	1864.381481	19.668045
57.523545	1863.335747	19.673063
57.332086	1861.138890	19.678080
57.589938	1866.334468	19.683098
58.142276	1888.199832	19.688115
57.965801	1886.565305	19.693133
58.521491	1881.313988	19.698151
58.183995	1879.972559	19.703168
58.302362	1866.305989	19.708186
58.441995	1877.968331	19.713203
58.528098	1867.879290	19.718221
58.312966	1850.119379	19.723239
58.101543	1851.230669	19.728256
58.317926	1860.483441	19.733274
58.255169	1880.019683	19.738291
57.869772	1875.338454	19.743309
58.552186	1866.653427	19.748327
58.333418	1882.566664	19.753344
58.662412	1880.384333	19.758362
58.765937	1884.306767	19.763379
58.714218	1874.872065	19.768397
58.610905	1868.917304	19.773415
58.548456	1884.311679	19.778432
58.807348	1891.608689	19.783450
59.205391	1902.361518	19.788467
58.973536	1900.141210	19.793485
59.401532	1902.246944	19.798503
59.367674	1908.607495	19.803520
59.494085	1892.550158	19.808538
59.767935	1895.553514	19.813555
59.478884	1893.052888	19.818573
59.421607	1866.325016	19.823591
59.182606	1876.156943	19.828608
59.489158	1888.387284	19.833626
59.660950	1906.429515	19.838643
59.524410	1901.836008	19.843661
59.780342	1894.027525	19.848679
59.525966	1895.317130	19.853696
59.370228	1896.545387	19.858714
59.878891	1893.983610	19.863731
59.734841	1886.073750	19.868749
59.683314	1887.368758	19.873767
59.376999	1895.106697	19.878784
59.476494	1900.237878	19.883802
59.836324	1908.890497	19.888819
59.947489	1918.381886	19.893837
60.630908	1913.089739	19.898855
60.402295	1916.975487	19.903872
60.551053	1913.591770	19.908890
60.416002	1914.086834	19.913907
60.197864	1924.143557	19.918925
60.627183	1905.881247	19.923943
60.271826	1920.573601	19.928960
60.563503	1905.141136	19.933978
60.697810	1917.531108	19.938995
60.412450	1918.006098	19.944013
60.811971	1911.832700	19.949031
60.773888	1927.043907	19.954048
60.927849	1936.594551	19.959066
61.147983	1934.048894	19.964083
61.258040	1925.628146	19.969101
61.439070	1935.800547	19.974119
60.977712	1938.438235	19.979136
61.254345	1936.006266	19.984154
61.530233	1934.702293	19.989171
61.052761	1939.714712	19.994189
61.401819	1924.285660	19.999207
60.986756	1941.271626	20.004224
61.045747	1935.526912	20.009242
61.541658	1921.683674	20.014259
61.499060	1930.265202	20.019277
61.853825	1925.783673	20.024295
61.380498	1936.758864	20.029312
61.462265	1951.609631	20.034330
61.715438	1960.233672	20.039347
61.807923	1962.518766	20.044365
62.243423	1963.064416	20.049383
62.119741	1952.455057	20.054400
62.014389	1958.155338	20.059418
62.189077	1957.120764	20.064435
62.058899	1960.026544	20.069453
62.424240	1957.891888	20.074471
62.136300	1963.493873	20.079488
62.192586	1964.298204	20.084506
62.310657	1958.432372	20.089523
62.061126	1960.943473	20.094541
62.665908	1959.708172	20.099559
62.770168	1979.666232	20.104576
63.094246	1976.377240	20.109594
62.917422	1964.239472	20.114611
62.478223	1954.111446	20.119629
62.640357	1967.201751	20.124647
63.028516	1975.804274	20.129664
63.133116	1987.900163	20.134682
63.576027	1967.427036	20.139699
63.069210	1969.131293	20.144717
63.096217	1962.867842	20.149735
63.439065	1960.529130	20.154752
63.333246	1973.058119	20.159770
63.549898	1972.122247	20.164787
63.373375	1960.752085	20.169805
63.336306	1973.200896	20.174823
63.317356	1972.892492	20.179840
63.343817	1983.374299	20.184858
63.923599	1969.819668	20.189875
63.808341	1972.159916	20.194893
64.341824	1982.224232	20.199911
63.962804	1981.323578	20.204928
64.090027	1973.837606	20.209946
64.228787	1975.813296	20.214963
63.843417	1977.185147	20.219981
63.996526	1961.092015	20.224999
63.674489	1979.167473	20.230016
63.826714	1976.657807	20.235034
63.811448	1971.991453	20.240051
63.871862	1976.339220	20.245069
63.927392	1981.963516	20.250087
64.245904	2006.705717	20.255104
64.295389	1999.447638	20.260122
64.316818	1993.063938	20.265139
64.287722	2011.800595	20.270157
64.533521	2000.992275	20.275175
64.435131	2005.937969	20.280192
64.485025	2021.327157	20.285210
64.822761	2030.412818	20.290227
64.826237	2024.289950	20.295245
64.913774	2025.504589	20.300263
64.966876	2031.135583	20.305280
65.214277	2027.696782	20.310298
65.106754	2025.662697	20.315315
64.841754	2030.785984	20.320333
65.028494	2015.170359	20.325351
65.250079	2014.110998	20.330368
65.298929	2040.879891	20.335386
65.753994	2044.862713	20.340403
65.505008	2050.213120	20.345421
65.361818	2042.214946	20.350439
65.640443	2041.676609	20.355456
65.725760	2054.826435	20.360474
65.978190	2036.423854	20.365491
65.800133	2054.312845	20.370509
65.933989	2045.351817	20.375527
66.114215	2040.833594	20.380544
65.772911	2048.905964	20.385562
65.880147	2048.439005	20.390579
66.111434	2044.927263	20.395597
66.246204	2041.929574	20.400615
66.110575	2039.618391	20.405632
65.939191	2053.520177	20.410650
66.168006	2050.079616	20.415667
66.134516	2065.678782	20.420685
66.419463	2070.258191	20.425703
66.613576	2067.966778	20.430720
66.509924	2079.658643	20.435738
66.806962	2073.267135	20.440755
66.952034	2079.154048	20.445773
66.920133	2071.526657	20.450791
66.957146	2061.124406	20.455808
66.854614	2077.241121	20.460826
67.015108	2060.984675	20.465843
66.706946	2072.720160	20.470861
66.828043	2065.947716	20.475879
66.875065	2073.443779	20.480896
67.144626	2096.441545	20.485914
67.757722	2086.318649	20.490931
67.705529	2098.414465	20.495949
67.854533	2094.670435	20.500967
67.801503	2090.890983	20.505984
67.560185	2093.188431	20.511002
67.908991	2083.065212	20.516019
67.801023	2086.599847	20.521037
67.898397	2082.709893	20.526055
68.369233	2079.955912	20.531072
67.846822	2089.339236	20.536090
68.311528	2077.503343	20.541107
68.204902	2085.127737	20.546125
68.167136	2090.059073	20.551143
68.196217	2085.552355	20.556160
67.843884	2088.284369	20.561178
68.113558	2086.621143	20.566195
68.038598	2083.004069	20.571213
68.153477	2095.452349	20.576231
68.600548	2071.151140	20.581248
68.132702	2095.826984	20.586266
68.876788	2099.098323	20.591283
68.903718	2110.096114	20.596301
68.819446	2113.240002	20.601319
68.897775	2102.692701	20.606336
68.937538	2111.393339	20.611354
69.205856	2115.461021	20.616371
69.084671	2104.731598	20.621389
69.061806	2109.128867	20.626407
69.255758	2102.187481	20.631424
69.294831	2110.707326	20.636442
69.360193	2098.990159	20.641459
68.841265	2106.763688	20.646477
69.308185	2102.600858	20.651495
69.709717	2106.892692	20.656512
69.080373	2115.415312	20.661530
69.108956	2106.765200	20.666547
69.062581	2136.986613	20.671565
69.254008	2138.769090	20.676583
69.632624	2132.470730	20.681600
69.505552	2135.558525	20.686618
69.758395	2158.176798	20.691635
70.191906	2161.776901	20.696653
70.102161	2159.742321	20.701671
70.135760	2163.086080	20.706688
70.502163	2165.498202	20.711706
70.658488	2158.014574	20.716723
70.713423	2160.871208	20.721741
70.606856	2161.055774	20.726759
70.747038	2160.885589	20.731776
70.580512	2160.069802	20.736794
70.667729	2155.652108	20.741811
70.797364	2157.991873	20.746829
70.824039	2157.132691	20.751847
70.863522	2147.887767	20.756864
70.719093	2158.901911	20.761882
71.128409	2155.080171	20.766899
71.070868	2152.009306	20.771917
70.713525	2156.197226	20.776935
71.218496	2148.274172	20.781952
71.009333	2154.501547	20.786970
70.946055	2144.204895	20.791987
71.171747	2150.407753	20.797005
70.915233	2163.475334	20.802023
71.345295	2166.184054	20.807040
71.234226	2169.513131	20.812058
71.184522	2170.489325	20.817075
71.507978	2176.745819	20.822093
71.497025	2188.811538	20.827111
72.029584	2195.426391	20.832128
71.749537	2201.285191	20.837146
71.452664	2203.247012	20.842163
72.031964	2192.926505	20.847181
72.143176	2198.689875	20.852199
72.224530	2189.684433	20.857216
72.310934	2199.972001	20.862234
72.216760	2188.723026	20.867251
72.124981	2204.463775	20.872269
72.182044	2222.466492	20.877287
72.412941	2209.764831	20.882304
72.686075	2224.917280	20.887322
72.696685	2226.354997	20.892339
72.875343	2221.777191	20.897357
72.815244	2226.255154	20.902375
72.810922	2220.924706	20.907392
73.158809	2219.562822	20.912410
73.443497	2218.437540	20.917427
73.464313	2222.780685	20.922445
73.382421	2228.437216	20.927463
73.464733	2221.655941	20.932480
73.132782	2220.426856	20.937498
73.298409	2209.874994	20.942515
73.351240	2213.473683	20.947533
73.375555	2214.964271	20.952551
73.457361	2217.523252	20.957568
73.212222	2228.043043	20.962586
73.490195	2234.641883	20.967603
73.658700	2247.898172	20.972621
73.430178	2249.160874	20.977639
73.773045	2243.161548	20.982656
73.777261	2237.142295	20.987674
73.523692	2253.086655	20.992691
74.293312	2260.580056	20.997709
74.118455	2272.380175	21.002727
74.519844	2268.337866	21.007744
74.339119	2270.657927	21.012762
74.673924	2264.629989	21.017779
74.573815	2257.473506	21.022797
74.498497	2265.415484	21.027815
74.676238	2254.882108	21.032832
74.660837	2271.237624	21.037850
74.441249	2279.780726	21.042867
74.679003	2256.696338	21.047885
74.698211	2262.251813	21.052903
74.981894	2274.899066	21.057920
75.184084	2294.679128	21.062938
75.434148	2293.359580	21.067955
75.443779	2295.056234	21.072973
75.622591	2291.474934	21.077991
75.837160	2292.500231	21.083008
75.649194	2284.970764	21.088026
75.533877	2288.608084	21.093043
75.943726	2276.653360	21.098061
75.611733	2285.274955	21.103079
75.658052	2279.145146	21.108096
75.700519	2286.200794	21.113114
75.817507	2281.993041	21.118131
76.149962	2278.307802	21.123149
76.019552	2283.992542	21.128167
76.263778	2274.375100	21.133184
76.075581	2281.890691	21.138202
75.999986	2285.351782	21.143219
76.283416	2286.141145	21.148237
75.933609	2288.686382	21.153255
76.568920	2293.953275	21.158272
76.423010	2309.651644	21.163290
76.155681	2318.270812	21.168307
76.676364	2307.393260	21.173325
76.523369	2319.130153	21.178343
76.607299	2306.226893	21.183360
76.518391	2311.489729	21.188378
76.786416	2318.474815	21.193395
77.049820	2321.441388	21.198413
77.016295	2328.516254	21.203431
77.209249	2328.004155	21.208448
77.102091	2333.973870	21.213466
76.934728	2331.965014	21.218483
77.431249	2328.309444	21.223501
77.295604	2328.453029	21.228519
77.312169	2339.238706	21.233536
77.495985	2334.203845	21.238554
77.618673	2344.629667	21.243571
78.014135	2359.382061	21.248589
77.740704	2361.319712	21.253607
78.182888	2350.595440	21.258624
78.257601	2355.332741	21.263642
78.043675	2355.289027	21.268659
78.112578	2350.458897	21.273677
78.063623	2356.418553	21.278695
78.304072	2354.978618	21.283712
78.513745	2347.508409	21.288730
78.186118	2348.281172	21.293747
78.508818	2337.339999	21.298765
78.435301	2347.447885	21.303783
78.514928	2338.616455	21.308800
78.880811	2362.673707	21.313818
78.816010	2369.372891	21.318835
78.883887	2368.547241	21.323853
78.965338	2375.322209	21.328871
78.940111	2362.476421	21.333888
79.376685	2373.729211	21.338906
79.392148	2369.040524	21.343923
79.400307	2360.719935	21.348941
79.428311	2365.196476	21.353959
79.374901	2361.985688	21.358976
79.386146	2377.158824	21.363994
79.286629	2373.997073	21.369011
79.913404	2359.156448	21.374029
79.487427	2369.322130	21.379047
79.604281	2386.142772	21.384064
79.910489	2386.723219	21.389082
80.146058	2387.783716	21.394099
80.182980	2392.220302	21.399117
80.236515	2391.081530	21.404135
80.449438	2395.836919	21.409152
80.497264	2386.201957	21.414170
80.182128	2397.433848	21.419187
80.462866	2388.843249	21.424205
80.315381	2388.551401	21.429223
80.335348	2394.184674	21.434240
80.532428	2397.225550	21.439258
80.891672	2411.754887	21.444275
81.020604	2410.277672	21.449293
80.856930	2424.715797	21.454311
81.158291	2421.622249	21.459328
81.175755	2422.474485	21.464346
81.071033	2433.321260	21.469363
81.251816	2426.764872	21.474381
81.051071	2425.111343	21.479399
81.225314	2422.340888	21.484416
81.545457	2423.858259	21.489434
81.301081	2419.729330	21.494451
81.348951	2413.702256	21.499469
81.270709	2419.944260	21.504487
81.615094	2432.496237	21.509504
81.974533	2438.162699	21.514522
81.685057	2446.027236	21.519539
82.261342	2435.444334	21.524557
81.826492	2445.569795	21.529575
82.010085	2455.578551	21.534592
82.053131	2442.163351	21.539610
82.058768	2438.890431	21.544627
82.402203	2445.536347	21.549645
82.253432	2465.560597	21.554663
82.207251	2469.764267	21.559680
82.430841	2470.611165	21.564698
82.022464	2473.693550	21.569715
82.344392	2481.083060	21.574733
82.886114	2498.377228	21.579751
82.495355	2507.832635	21.584768
83.011782	2493.643436	21.589786
83.153942	2500.296305	21.594803
83.280521	2488.915147	21.599821
83.298320	2501.506679	21.604839
83.097153	2490.691406	21.609856
83.328048	2490.269212	21.614874
83.561631	2501.696839	21.619891
84.305205	2503.428282	21.624909
83.962527	2498.813970	21.629927
83.984144	2493.373100	21.634944
84.121919	2491.973910	21.639962
83.853345	2495.106368	21.644979
83.629796	2493.707378	21.649997
83.924086	2516.033295	21.655015
83.915066	2519.045712	21.660032
84.250620	2525.394031	21.665050
84.265828	2527.214098	21.670067
84.058863	2528.854864	21.675085
84.315549	2518.752329	21.680103
84.091220	2527.106771	21.685120
84.308735	2534.711958	21.690138
84.111599	2544.731149	21.695155
84.631654	2545.876860	21.700173
84.587856	2553.817115	21.705191
84.662571	2564.680994	21.710208
84.977560	2567.898171	21.715226
85.079506	2569.345740	21.720243
85.570514	2571.641317	21.725261
85.729276	2567.841338	21.730279
85.738066	2575.711866	21.735296
85.791983	2560.525851	21.740314
85.992667	2559.343937	21.745331
86.152812	2554.672233	21.750349
85.988580	2543.003120	21.755367
85.863707	2531.711580	21.760384
85.985473	2509.254085	21.765402
86.142862	2528.355734	21.770419
86.306095	2521.456017	21.775437
86.192377	2522.656386	21.780455
86.137661	2522.643126	21.785472
86.147663	2542.150564	21.790490
86.237400	2547.402301	21.795507
86.343560	2544.917977	21.800525
86.044843	2549.622865	21.805543
85.940475	2562.377085	21.810560
86.356354	2573.179487	21.815578
86.397773	2579.378094	21.820595
86.630041	2579.334801	21.825613
86.825081	2583.032034	21.830631
86.868262	2585.337675	21.835648
87.130926	2583.332572	21.840666
86.679785	2575.251068	21.845683
87.309572	2597.541701	21.850701
87.115659	2606.345184	21.855719
87.498462	2607.253222	21.860736
87.588558	2599.713858	21.865754
87.378840	2596.944822	21.870771
87.591998	2606.261513	21.875789
87.600384	2611.070827	21.880807
87.985342	2606.268083	21.885824
88.258652	2627.328792	21.890842
88.052004	2638.278496	21.895859
88.521608	2621.579638	21.900877
88.475623	2627.933785	21.905895
88.071619	2624.361182	21.910912
88.573953	2626.660468	21.915930
88.401228	2629.076842	21.920947
88.505152	2628.759055	21.925965
88.676002	2621.345238	21.930983
89.015291	2625.725812	21.936000
89.067158	2622.221308	21.941018
88.823151	2623.634383	21.946035
88.751713	2619.561194	21.951053
88.967027	2621.940071	21.956071
88.980720	2623.607799	21.961088
89.304527	2626.952580	21.966106
89.162049	2638.655017	21.971123
89.045610	2645.200529	21.976141
89.433517	2646.957246	21.981159
89.298129	2658.941731	21.986176
89.605335	2644.572592	21.991194
89.758210	2644.799167	21.996211
89.703099	2662.529289	22.001229
89.930583	2668.518139	22.006247
89.714620	2675.206173	22.011264
90.215093	2677.884103	22.016282
89.927424	2682.982913	22.021299
89.739279	2673.242236	22.026317
90.063363	2682.294305	22.031335
90.276392	2691.813219	22.036352
90.757109	2697.483256	22.041370
90.546803	2702.945716	22.046387
90.962979	2698.623275	22.051405
91.068122	2697.684691	22.056423
90.837201	2700.086760	22.061440
91.301450	2687.842223	22.066458
91.339936	2694.814542	22.071475
91.338249	2695.288363	22.076493
91.136520	2687.754588	22.081511
91.166680	2691.419149	22.086528
91.148513	2683.793180	22.091546
91.445999	2701.305089	22.096563
91.520719	2693.794872	22.101581
91.298568	2687.806811	22.106599
91.309042	2707.824876	22.111616
91.816088	2711.578575	22.116634
91.671569	2712.897136	22.121651
91.944762	2720.675240	22.126669
91.678166	2725.684183	22.131687
91.690917	2741.028929	22.136704
92.018540	2736.151123	22.141722
92.092929	2757.314533	22.146739
92.172951	2750.346962	22.151757
92.616996	2741.774950	22.156775
92.556857	2757.324833	22.161792
93.154799	2761.769604	22.166810
93.294334	2773.640337	22.171827
93.068158	2766.398305	22.176845
93.170979	2755.507615	22.181863
93.315970	2765.236430	22.186880
93.861637	2765.600945	22.191898
93.650390	2755.334535	22.196915
93.648415	2735.422886	22.201933
93.783026	2726.584813	22.206951
93.231567	2744.306088	22.211968
93.543668	2744.581211	22.216986
93.882042	2752.818521	22.222003
94.060035	2752.965581	22.227021
94.030179	2756.926040	22.232039
93.893276	2757.725041	22.237056
94.040812	2748.901411	22.242074
93.982818	2758.748326	22.247091
94.285934	2750.592067	22.252109
94.583806	2751.607261	22.257127
94.125595	2759.096935	22.262144
94.471709	2783.780217	22.267162
94.418929	2784.503666	22.272179
94.645879	2788.865236	22.277197
94.714086	2797.350161	22.282215
94.866619	2794.431291	22.287232
94.942312	2785.449983	22.292250
94.879347	2793.030814	22.297267
95.017752	2802.943189	22.302285
95.457842	2805.277601	22.307303
95.347349	2811.379400	22.312320
95.480028	2803.020611	22.317338
95.592504	2805.675487	22.322355
95.709652	2818.399326	22.327373
95.867826	2813.059268	22.332391
95.643036	2819.632362	22.337408
95.788399	2806.754258	22.342426
95.880126	2818.800193	22.347443
95.736734	2809.830208	22.352461
96.131664	2816.899914	22.357479
95.919121	2836.763368	22.362496
95.915193	2846.757463	22.367514
96.109344	2840.800488	22.372531
96.288635	2836.535447	22.377549
96.492334	2858.982526	22.382567
96.339775	2866.350362	22.387584
96.905389	2857.334933	22.392602
97.179475	2865.002066	22.397619
96.840300	2863.601812	22.402637
97.116785	2850.485666	22.407655
97.042542	2856.779133	22.412672
97.268377	2867.737127	22.417690
97.582380	2877.392657	22.422707
97.956440	2881.797656	22.427725
98.427663	2881.072054	22.432743
97.846116	2889.231960	22.437760
97.816424	2881.918422	22.442778
98.142200	2882.313287	22.447795
97.975720	2878.924558	22.452813
98.166268	2883.329717	22.457831
98.109632	2883.769044	22.462848
98.145492	2886.149052	22.467866
98.462013	2876.068979	22.472883
98.186445	2878.729901	22.477901
98.752562	2873.865147	22.482919
98.611078	2888.945970	22.487936
98.493374	2892.495723	22.492954
98.708801	2888.604822	22.497971
98.497482	2901.706755	22.502989
98.896899	2899.541366	22.508007
98.866999	2903.566371	22.513024
98.841071	2916.272209	22.518042
99.263016	2931.421334	22.523059
99.479748	2937.804514	22.528077
99.803098	2939.430766	22.533095
99.378624	2942.322313	22.538112
99.519831	2933.297430	22.543130
99.487992	2932.910830	22.548147
99.850082	2955.458653	22.553165
100.026794	2955.110374	22.558183
99.826790	2960.864681	22.563200
100.063560	2957.710531	22.568218
100.344215	2962.784885	22.573235
100.155251	2961.610014	22.578253
100.656959	2955.129641	22.583271
100.470795	2957.062892	22.588288
100.447675	2969.187831	22.593306
101.154914	2977.124969	22.598323
100.597931	2998.268275	22.603341
100.709888	2985.792566	22.608359
101.029209	2998.430049	22.613376
101.062170	2986.829031	22.618394
101.018865	2992.791191	22.623411
101.245033	2983.655980	22.628429
101.700594	2985.855024	22.633447
101.880710	3009.750261	22.638464
102.030016	3004.383230	22.643482
102.146461	2985.108368	22.648499
101.877813	2979.723042	22.653517
102.369416	2993.461795	22.658535
102.117432	2993.449314	22.663552
101.692318	2992.398621	22.668570
102.281106	2996.079582	22.673587
101.908450	2996.389964	22.678605
102.196513	3006.169278	22.683623
102.339877	3022.054327	22.688640
102.251211	3026.924090	22.693658
102.520858	3024.185506	22.698675
102.344035	3040.133430	22.703693
102.593832	3031.947762	22.708711
102.479303	3042.931059	22.713728
102.683096	3051.777579	22.718746
102.938492	3052.257612	22.723763
103.049995	3058.847193	22.728781
103.721873	3075.060194	22.733799
103.834636	3087.090411	22.738816
104.336334	3081.873246	22.743834
104.238032	3075.616713	22.748851
103.675515	3061.027955	22.753869
104.303395	3069.188605	22.758887
104.288224	3076.618803	22.763904
104.223491	3085.646602	22.768922
104.690275	3073.307738	22.773939
104.351468	3087.245070	22.778957
104.540086	3073.764388	22.783975
104.370278	3079.079730	22.788992
104.444873	3088.919883	22.794010
104.653070	3081.298512	22.799027
104.625525	3080.529727	22.804045
104.574134	3090.165794	22.809063
104.562879	3101.463034	22.814080
104.768071	3105.744005	22.819098
104.853152	3103.372284	22.824115
104.979041	3129.814686	22.829133
105.515346	3129.741005	22.834151
105.572389	3124.526296	22.839168
105.571804	3134.356443	22.844186
106.191969	3126.045591	22.849203
105.949960	3128.058561	22.854221
106.023380	3120.080311	22.859239
106.366407	3129.891847	22.864256
106.270015	3120.738766	22.869274
106.398643	3127.110122	22.874291
106.442883	3132.720932	22.879309
106.594568	3126.206629	22.884327
106.907993	3131.874412	22.889344
106.746680	3140.237245	22.894362
107.077485	3142.847144	22.899379
106.877699	3147.029880	22.904397
107.095855	3145.149790	22.909415
107.173919	3149.735791	22.914432
107.084216	3148.821170	22.919450
107.233363	3152.278879	22.924467
107.128319	3147.659499	22.929485
107.240596	3139.605823	22.934503
107.377541	3166.450837	22.939520
107.476182	3175.384993	22.944538
107.546530	3169.612812	22.949555
107.621786	3179.677887	22.954573
107.679015	3179.084361	22.959591
107.863516	3191.449326	22.964608
107.947586	3206.535413	22.969626
108.227155	3197.356944	22.974643
108.369315	3208.951521	22.979661
108.537352	3208.289983	22.984679
108.728257	3230.553252	22.989696
108.773327	3226.333099	22.994714
109.266474	3226.749270	22.999731
108.912942	3236.028515	23.004749
109.181674	3229.796768	23.009767
109.334940	3225.792195	23.014784
109.364630	3225.274640	23.019802
109.417898	3224.558249	23.024819
109.308125	3234.450710	23.029837
109.642812	3249.563740	23.034855
109.946646	3250.173711	23.039872
109.600491	3258.073676	23.044890
110.179217	3251.329184	23.049907
110.149497	3257.527625	23.054925
110.164402	3258.587193	23.059943
110.179976	3251.283557	23.064960
110.350491	3248.095074	23.069978
110.745832	3279.111317	23.074995
110.361149	3289.033493	23.080013
110.769173	3293.484333	23.085031
110.930147	3276.577515	23.090048
110.427531	3286.335217	23.095066
110.777141	3283.740368	23.100083
110.737655	3296.161590	23.105101
111.079895	3304.736050	23.110119
111.442208	3304.947332	23.115136
111.405816	3309.004948	23.120154
111.739884	3300.564208	23.125171
111.847072	3311.251988	23.130189
112.061374	3306.649284	23.135207
112.075798	3297.412346	23.140224
111.791690	3299.494193	23.145242
112.041685	3305.735364	23.150259
112.251406	3328.899586	23.155277
112.125211	3319.569427	23.160295
112.330942	3325.503812	23.165312
112.219642	3324.230000	23.170330
112.488089	3320.892164	23.175347
112.456396	3328.854508	23.180365
112.651057	3341.760735	23.185383
113.015092	3351.620987	23.190400
112.846707	3354.763606	23.195418
113.020135	3355.742055	23.200435
112.904392	3357.525685	23.205453
113.143991	3370.947077	23.210471
113.634799	3382.283254	23.215488
113.416905	3389.386459	23.220506
113.998449	3380.848003	23.225523
113.680706	3379.983101	23.230541
113.878876	3369.201034	23.235559
114.301406	3371.289777	23.240576
114.071318	3404.218348	23.245594
114.274494	3395.651329	23.250611
114.387847	3403.128848	23.255629
114.517762	3397.762406	23.260647
114.737146	3402.616210	23.265664
114.679420	3408.369243	23.270682
114.735075	3396.690339	23.275699
115.261668	3410.168263	23.280717
115.297277	3423.960471	23.285735
115.390485	3419.084424	23.290752
115.415775	3425.236407	23.295770
115.459550	3424.206091	23.300787
115.728841	3418.373772	23.305805
115.611539	3423.740647	23.310823
115.812709	3425.568145	23.315840
115.613703	3423.649133	23.320858
115.859912	3433.187629	23.325875
116.196267	3445.799189	23.330893
116.114751	3445.946736	23.335911
116.449048	3446.976627	23.340928
116.174589	3455.248342	23.345946
116.457777	3451.639107	23.350963
116.245862	3454.576305	23.355981
116.636800	3462.891379	23.360999
117.121998	3460.696502	23.366016
117.050752	3464.883217	23.371034
117.389989	3455.981398	23.376051
117.548790	3465.655776	23.381069
117.454663	3466.532947	23.386087
117.833036	3463.265651	23.391104
117.638802	3456.560939	23.396122
117.759889	3444.973822	23.401139
117.868249	3448.995024	23.406157
117.848771	3464.174189	23.411175
118.137122	3474.797805	23.416192
118.112422	3484.413356	23.421210
118.182502	3472.930317	23.426227
118.365904	3482.083982	23.431245
118.196783	3486.331146	23.436263
118.646086	3488.303939	23.441280
118.349675	3485.727900	23.446298
118.422317	3494.864624	23.451315
118.879735	3504.143731	23.456333
118.987999	3509.536026	23.461351
119.169804	3511.310773	23.466368
118.881689	3508.414043	23.471386
119.485812	3522.055123	23.476403
119.434086	3529.742310	23.481421
119.735080	3537.141208	23.486439
119.677434	3535.420679	23.491456
119.743442	3532.558725	23.496474
119.916680	3537.513539	23.501491
119.832111	3544.734004	23.506509
120.170002	3558.709403	23.511527
120.888191	3568.595927	23.516544
120.377628	3559.709197	23.521562
121.125189	3555.723832	23.526579
120.928266	3562.885919	23.531597
120.743541	3565.043989	23.536615
121.215067	3554.185161	23.541632
120.956020	3551.342783	23.546650
121.308531	3554.196294	23.551667
121.151282	3556.377512	23.556685
121.247310	3576.637204	23.561703
121.375954	3581.781639	23.566720
121.256424	3585.616604	23.571738
121.670967	3579.016923	23.576755
121.901095	3595.787863	23.581773
121.678472	3610.035182	23.586791
121.915464	3618.856303	23.591808
121.932186	3608.589908	23.596826
122.388564	3626.814658	23.601843
122.598497	3632.533753	23.606861
122.657880	3634.810232	23.611879
122.849276	3637.987578	23.616896
122.729292	3642.508560	23.621914
123.248699	3633.846143	23.626931
123.260084	3629.215911	23.631949
123.223127	3636.574353	23.636967
123.510225	3630.737538	23.641984
123.353066	3642.578415	23.647002
123.434481	3670.280397	23.652019
123.773511	3662.943859	23.657037
123.781334	3664.935943	23.662055
124.008700	3654.044391	23.667072
123.626095	3669.333588	23.672090
123.796683	3674.638131	23.677107
124.158610	3676.713772	23.682125
124.074577	3691.693440	23.687143
124.598391	3684.937844	23.692160
124.717331	3681.512854	23.697178
124.679260	3684.433389	23.702195
124.848245	3682.367565	23.707213
124.552763	3704.089256	23.712231
125.175345	3702.054936	23.717248
125.345853	3712.383654	23.722266
125.320773	3693.169757	23.727283
125.080595	3715.630723	23.732301
125.209005	3717.461207	23.737319
125.536372	3717.999800	23.742336
125.682167	3737.595736	23.747354
125.672887	3740.997825	23.752371
125.560341	3748.947330	23.757389
125.715867	3768.499279	23.762407
126.491162	3771.545006	23.767424
126.314154	3779.150825	23.772442
126.445374	3773.049331	23.777459
127.007317	3784.496409	23.782477
126.893671	3790.434712	23.787495
127.157059	3793.580947	23.792512
127.444532	3792.090117	23.797530
127.149059	3796.637555	23.802547
127.372495	3799.060960	23.807565
127.256193	3806.572158	23.812583
127.579248	3805.077226	23.817600
127.582708	3823.481421	23.822618
127.546091	3831.548658	23.827635
127.963018	3823.817319	23.832653
128.003683	3827.506449	23.837671
128.068978	3826.955664	23.842688
128.464539	3843.023223	23.847706
128.523780	3847.970363	23.852723
128.725893	3848.400712	23.857741
128.671477	3852.806683	23.862759
129.184233	3845.680702	23.867776
129.016497	3846.583004	23.872794
129.002234	3846.509801	23.877811
129.580792	3856.077391	23.882829
129.214114	3870.489525	23.887847
129.426404	3877.554264	23.892864
129.487457	3878.531789	23.897882
129.399554	3873.641991	23.902899
130.048877	3876.459254	23.907917
129.559094	3897.290280	23.912935
129.906976	3893.717821	23.917952
130.204217	3904.389105	23.922970
130.532263	3902.695137	23.927987
130.848751	3896.460216	23.933005
130.608806	3906.300729	23.938023
130.832195	3908.803610	23.943040
130.684230	3917.727984	23.948058
130.938784	3923.244207	23.953075
131.376862	3919.013895	23.958093
131.392845	3918.445010	23.963111
131.449951	3915.601707	23.968128
131.714120	3929.832288	23.973146
131.697029	3931.590817	23.978163
131.677255	3919.038562	23.983181
131.681664	3937.230358	23.988199
131.750533	3944.745140	23.993216
131.956596	3956.349789	23.998234
132.190301	3948.127634	24.003251
132.287537	3946.967616	24.008269
132.276901	3970.802807	24.013287
132.577963	3974.470121	24.018304
132.760363	3983.947569	24.023322
132.637988	3982.276639	24.028339
133.004006	3970.840420	24.033357
133.224521	3991.181526	24.038375
133.429043	4008.801084	24.043392
133.335494	3996.532703	24.048410
133.350066	4009.129196	24.053427
133.607769	3993.954037	24.058445
133.204698	4010.806751	24.063463
133.629196	4027.162529	24.068480
134.001919	4027.626253	24.073498
134.023196	4042.315737	24.078515
134.023856	4053.935907	24.083533
134.367239	4065.775192	24.088551
134.440616	4061.559725	24.093568
134.983783	4054.951126	24.098586
134.895973	4068.291636	24.103603
135.234650	4079.913784	24.108621
135.531616	4084.896256	24.113639
135.854444	4076.424614	24.118656
135.880162	4084.384507	24.123674
135.444243	4082.383612	24.128691
135.958986	4084.540358	24.133709
136.143724	4079.455984	24.138727
135.956970	4068.726914	24.143744
136.298471	4072.398031	24.148762
135.896836	4079.710219	24.153779
136.697931	4091.542622	24.158797
136.504560	4099.414740	24.163815
136.905510	4096.330930	24.168832
136.589934	4094.546837	24.173850
136.549862	4090.692427	24.178867
136.757213	4093.005957	24.183885
136.873589	4109.412531	24.188903
136.865554	4110.926564	24.193920
137.438678	4130.008078	24.198938
137.390304	4124.029472	24.203955
137.714802	4131.413126	24.208973
137.766525	4150.208866	24.213991
137.963593	4158.305100	24.219008
138.081650	4153.785131	24.224026
137.721880	4150.344324	24.229043
138.307723	4166.087696	24.234061
138.397326	4170.374827	24.239079
138.265691	4188.850580	24.244096
138.726758	4181.683124	24.249114
138.875722	4191.600267	24.254131
138.974413	4187.017297	24.259149
139.132064	4194.801245	24.264167
139.611736	4198.656466	24.269184
139.988665	4197.674454	24.274202
139.817578	4209.759509	24.279219
139.759309	4190.589584	24.284237
139.901604	4193.458650	24.289255
139.942235	4192.304492	24.294272
140.254336	4186.623948	24.299290
140.205785	4199.290455	24.304307
140.427962	4212.231612	24.309325
140.509102	4224.441658	24.314343
140.544541	4227.478805	24.319360
141.054436	4223.534311	24.324378
140.739146	4227.427401	24.329395
140.766015	4240.997577	24.334413
140.877768	4250.935640	24.339431
141.146580	4253.259849	24.344448
141.192754	4247.382542	24.349466
141.483606	4275.127794	24.354483
141.899508	4278.820141	24.359501
141.973751	4283.101888	24.364519
141.920985	4292.351144	24.369536
142.237069	4279.419356	24.374554
142.356180	4297.814361	24.379571
142.503897	4309.627616	24.384589
142.755773	4319.238163	24.389607
142.527155	4308.208796	24.394624
142.601681	4305.935324	24.399642
142.624081	4336.081094	24.404659
142.753992	4341.789627	24.409677
142.839898	4348.005492	24.414695
143.126327	4348.151019	24.419712
143.829154	4365.580638	24.424730
143.379308	4367.484525	24.429747
143.552584	4362.629226	24.434765
144.386495	4387.305103	24.439783
144.249739	4396.377445	24.444800
144.575785	4381.836836	24.449818
144.698790	4383.308765	24.454835
144.781942	4378.996464	24.459853
144.875057	4385.320541	24.464871
144.795399	4385.076830	24.469888
145.325929	4394.003444	24.474906
145.172752	4408.349021	24.479923
145.377207	4412.621844	24.484941
145.594502	4407.243464	24.489959
145.626729	4417.599449	24.494976
145.790304	4411.517706	24.499994
145.645528	4416.809083	24.505011
146.229370	4419.713205	24.510029
146.392004	4432.212508	24.515047
146.123664	4434.794670	24.520064
146.542059	4427.380595	24.525082
146.415733	4441.476485	24.530099
146.443733	4444.758728	24.535117
146.705597	4449.050729	24.540135
146.776472	4459.665686	24.545152
146.930886	4455.212988	24.550170
146.901737	4461.760337	24.555187
147.221370	4483.904300	24.560205
147.436441	4491.702851	24.565223
147.269157	4505.363227	24.570240
147.560848	4490.197086	24.575258
147.626168	4505.554968	24.580275
147.819609	4519.168070	24.585293
147.826426	4510.434260	24.590311
147.797399	4536.402015	24.595328
148.423242	4543.077034	24.600346
148.436499	4546.640916	24.605363
148.931038	4547.629611	24.610381
148.938405	4566.244155	24.615399
149.024504	4575.850622	24.620416
149.206813	4567.124198	24.625434
149.313100	4576.777007	24.630451
149.433987	4596.169597	24.635469
149.837282	4594.495023	24.640487
149.956276	4597.149976	24.645504
150.043360	4596.687729	24.650522
150.113962	4599.141931	24.655539
150.645789	4620.843201	24.660557
150.688885	4620.859182	24.665575
150.698741	4623.449727	24.670592
150.898901	4612.187353	24.675610
151.243174	4631.324105	24.680627
151.219438	4612.513925	24.685645
151.353320	4614.670119	24.690663
151.720575	4645.553718	24.695680
151.651012	4648.387425	24.700698
151.869545	4646.050820	24.705715
151.902063	4642.489133	24.710733
151.921616	4648.768412	24.715751
151.717388	4664.478600	24.720768
151.928862	4656.906241	24.725786
152.227084	4669.848265	24.730803
152.248364	4683.314328	24.735821
152.622550	4704.924429	24.740839
152.795152	4699.884258	24.745856
153.244167	4707.378155	24.750874
152.900640	4709.895258	24.755891
153.179703	4727.362196	24.760909
153.868047	4720.255006	24.765927
153.634538	4736.211448	24.770944
153.866464	4727.066373	24.775962
153.935119	4732.474090	24.780979
153.785058	4735.957069	24.785997
154.140871	4737.622412	24.791015
154.227000	4756.992436	24.796032
154.509804	4762.668104	24.801050
154.520656	4769.876315	24.806067
154.307574	4764.684426	24.811085
154.900415	4785.874313	24.816103
154.877811	4794.757203	24.821120
155.180026	4789.405266	24.826138
155.210468	4803.694417	24.831155
155.168974	4810.562495	24.836173
155.557338	4829.086733	24.841191
155.681973	4824.428628	24.846208
155.874188	4836.243867	24.851226
155.880097	4846.041087	24.856243
155.746980	4843.454498	24.861261
156.641588	4860.843121	24.866279
156.583084	4881.229950	24.871296
156.694402	4869.789593	24.876314
156.560886	4881.287061	24.881331
156.682208	4891.453744	24.886349
157.129085	4899.756794	24.891367
157.161059	4903.148641	24.896384
157.289422	4921.030033	24.901402
157.795071	4930.971050	24.906419
158.361990	4927.737888	24.911437
158.429761	4925.909876	24.916455
158.449167	4928.738105	24.921472
158.561935	4931.035383	24.926490
158.977999	4921.085158	24.931507
159.053231	4920.208634	24.936525
159.379820	4913.478425	24.941543
159.361174	4923.717009	24.946560
159.620779	4932.697378	24.951578
159.571687	4951.075965	24.956595
159.270040	4942.808810	24.961613
159.749735	4939.390521	24.966631
159.293860	4949.119830	24.971648
159.826810	4953.246824	24.976666
160.067219	4969.255400	24.981683
160.382292	4970.175192	24.986701
160.443702	4970.634307	24.991719
160.211953	4993.709494	24.996736
160.523084	4994.475725	25.001754
160.544809	4996.240779	25.006771
160.782274	5011.810112	25.011789
161.369251	5023.546829	25.016807
161.284622	5033.268926	25.021824
161.434376	5027.324444	25.026842
161.487332	5038.143284	25.031859
161.634222	5057.371852	25.036877
162.015355	5056.245155	25.041895
161.815509	5071.420125	25.046912
162.002446	5064.285726	25.051930
162.074995	5090.761415	25.056947
162.299485	5088.002910	25.061965
162.767628	5093.528007	25.066983
162.674278	5093.178689	25.072000
162.987470	5115.340367	25.077018
163.176500	5109.938705	25.082035
163.189369	5117.769042	25.087053
163.330086	5123.069436	25.092071
163.565271	5142.101524	25.097088
163.908651	5149.165647	25.102106
164.118801	5149.756033	25.107123
163.978123	5161.063693	25.112141
164.027793	5165.832649	25.117159
164.319406	5174.125995	25.122176
164.317143	5180.375152	25.127194
164.500362	5188.683428	25.132211
164.617770	5208.468371	25.137229
165.047960	5201.656219	25.142247
164.992629	5220.906229	25.147264
165.444774	5234.754094	25.152282
165.796153	5234.606854	25.157299
165.595938	5251.559229	25.162317
166.137445	5232.957084	25.167335
166.443793	5269.177685	25.172352
166.432625	5258.279714	25.177370
166.644797	5266.844604	25.182387
166.926946	5271.103721	25.187405
167.351731	5260.235367	25.192423
166.834839	5271.684124	25.197440
167.406553	5264.923330	25.202458
167.550066	5284.376158	25.207475
167.281442	5298.351586	25.212493
167.951636	5283.318602	25.217511
167.832733	5295.942986	25.222528
167.622937	5295.542211	25.227546
168.062377	5306.593858	25.232563
168.165603	5327.038909	25.237581
168.130005	5318.840049	25.242599
168.205514	5329.807342	25.247616
168.708369	5341.597850	25.252634
168.876194	5351.179994	25.257651
168.496294	5357.271515	25.262669
169.117107	5375.398284	25.267687
169.265898	5375.829319	25.272704
169.265984	5400.577702	25.277722
169.884702	5403.501643	25.282739
169.970659	5403.541474	25.287757
169.958163	5409.362028	25.292775
170.047646	5434.700410	25.297792
170.450091	5434.410499	25.302810
170.420612	5429.196181	25.307827
170.242032	5455.025762	25.312845
171.161388	5454.682547	25.317863
171.192130	5461.172015	25.322880
171.324691	5461.685099	25.327898
171.676918	5466.405916	25.332915
171.686257	5483.263783	25.337933
172.473913	5474.130348	25.342951
172.523761	5490.891293	25.347968
172.103114	5471.688573	25.352986
172.668189	5482.374168	25.358003
172.501426	5489.069788	25.363021
172.553562	5483.980114	25.368039
172.509758	5485.761968	25.373056
172.765071	5508.639152	25.378074
172.868531	5495.645010	25.383091
172.676526	5509.945137	25.388109
173.289645	5526.279605	25.393127
173.330061	5532.819485	25.398144
173.463950	5537.451621	25.403162
173.862756	5559.851283	25.408179
173.828669	5567.745203	25.413197
174.395573	5563.415223	25.418215
174.565548	5573.428292	25.423232
174.824696	5586.825788	25.428250
175.118589	5592.927202	25.433267
174.850666	5587.433795	25.438285
175.296990	5599.123383	25.443303
175.073152	5612.627015	25.448320
175.125164	5610.177560	25.453338
175.655890	5619.000264	25.458355
175.594470	5638.892182	25.463373
176.269709	5634.663705	25.468391
176.387059	5647.201946	25.473408
176.358566	5652.745858	25.478426
176.620642	5662.938626	25.483443
176.806271	5670.073783	25.488461
177.200993	5660.682683	25.493479
177.540242	5672.836262	25.498496
177.368023	5671.855961	25.503514
177.766755	5671.099325	25.508531
177.628503	5694.642963	25.513549
177.844143	5690.627782	25.518567
177.938895	5695.734309	25.523584
178.167987	5699.528401	25.528602
178.451906	5714.625330	25.533619
178.602913	5728.873343	25.538637
178.783731	5723.693052	25.543655
178.809316	5725.743161	25.548672
178.605260	5743.581782	25.553690
179.184897	5753.084373	25.558707
178.925577	5756.604678	25.563725
179.169029	5776.637778	25.568743
179.520551	5780.009565	25.573760
179.680564	5787.967851	25.578778
180.251164	5806.266801	25.583795
180.068092	5816.823310	25.588813
180.299405	5816.030419	25.593831
180.537014	5844.921597	25.598848
180.312160	5839.114401	25.603866
181.006761	5838.680352	25.608883
180.960170	5849.584104	25.613901
180.946245	5877.178782	25.618919
181.324389	5875.765347	25.623936
181.239371	5873.801870	25.628954
181.777243	5895.124072	25.633971
182.164792	5899.075476	25.638989
182.862261	5890.635123	25.644007
182.656632	5897.366233	25.649024
182.589917	5889.731387	25.654042
183.254152	5886.297629	25.659059
182.995416	5896.274630	25.664077
183.229397	5913.510999	25.669095
183.455350	5908.591726	25.674112
183.433346	5912.883000	25.679130
183.546047	5918.992196	25.684148
183.423266	5925.215251	25.689165
183.854161	5935.814001	25.694183
183.788655	5947.183444	25.699200
184.209914	5965.030423	25.704218
184.590848	5965.533825	25.709236
184.343815	5972.482416	25.714253
184.639057	5992.508340	25.719271
185.064739	6003.658690	25.724288
185.217399	6014.188564	25.729306
185.473885	6014.492306	25.734324
185.896864	6037.096544	25.739341
186.066551	6040.216513	25.744359
185.907478	6030.332065	25.749376
186.191333	6038.199149	25.754394
186.811718	6043.623239	25.759412
186.570365	6051.765242	25.764429
186.560666	6063.152626	25.769447
187.146330	6070.933061	25.774464
187.124599	6089.517978	25.779482
187.593411	6088.038143	25.784500
187.669642	6100.381130	25.789517
187.744094	6078.647962	25.794535
188.063822	6100.810871	25.799552
188.099564	6109.536555	25.804570
188.302304	6120.190695	25.809588
188.745334	6121.008344	25.814605
188.180729	6120.044150	25.819623
188.665167	6137.796298	25.824640
189.005697	6144.377508	25.829658
189.107079	6144.355876	25.834676
189.177823	6177.272578	25.839693
189.169783	6182.467257	25.844711
189.558266	6178.909817	25.849728
189.607647	6220.904436	25.854746
189.855584	6204.756926	25.859764
190.033304	6226.356531	25.864781
190.276988	6238.718569	25.869799
191.474604	6222.715459	25.874816
191.983532	6221.768145	25.879834
192.022851	6207.915812	25.884852
192.052640	6210.955056	25.889869
192.394917	6208.774716	25.894887
192.504345	6194.113449	25.899904
192.245215	6174.014696	25.904922
192.432173	6165.687835	25.909940
192.752917	6181.425298	25.914957
192.733661	6187.680737	25.919975
192.817164	6185.333166	25.924992
192.910934	6201.751973	25.930010
193.068548	6191.307112	25.935028
193.315227	6193.010485	25.940045
193.134955	6193.168291	25.945063
193.713694	6202.904986	25.950080
193.527291	6236.866716	25.955098
193.581903	6230.487684	25.960116
193.804386	6240.660416	25.965133
194.159552	6245.926242	25.970151
194.380423	6248.735982	25.975168
194.337596	6266.186833	25.980186
194.492268	6267.557136	25.985204
194.693486	6278.081031	25.990221
194.794315	6299.742568	25.995239
195.187982	6311.644893	26.000256
195.076735	6321.214727	26.005274
195.476316	6332.738481	26.010292
195.646310	6343.992008	26.015309
195.718018	6360.744163	26.020327
196.426468	6371.325731	26.025344
196.274603	6381.144402	26.030362
196.609942	6389.493622	26.035380
196.996055	6405.495484	26.040397
196.967207	6409.120816	26.045415
197.447086	6403.185310	26.050432
197.586570	6437.379568	26.055450
197.765449	6420.466294	26.060468
198.023802	6433.915043	26.065485
198.344916	6449.114584	26.070503
198.642099	6446.636921	26.075520
198.598486	6461.599583	26.080538
198.773351	6449.545210	26.085556
198.958495	6469.723086	26.090573
199.352280	6482.691603	26.095591
199.293114	6483.219555	26.100608
199.217750	6483.772119	26.105626
199.585529	6501.821035	26.110644
199.817274	6520.042721	26.115661
199.745571	6518.725334	26.120679
200.184446	6534.479746	26.125696
200.356365	6550.182321	26.130714
200.845166	6555.264880	26.135732
201.170420	6570.331709	26.140749
201.053053	6587.939589	26.145767
201.577040	6571.587170	26.150784
201.651143	6585.942684	26.155802
201.596465	6593.152791	26.160820
202.044395	6592.745469	26.165837
201.612092	6615.569555	26.170855
201.927428	6617.471315	26.175872
201.970969	6630.325068	26.180890
202.269407	6624.732325	26.185908
202.417019	6649.072972	26.190925
202.618196	6674.387807	26.195943
203.064778	6666.222267	26.200960
203.271009	6687.559938	26.205978
203.695164	6692.536408	26.210996
203.983767	6695.721746	26.216013
204.152590	6689.154365	26.221031
204.325129	6710.056056	26.226048
204.421888	6724.411239	26.231066
204.590461	6708.416669	26.236084
205.370550	6738.020910	26.241101
205.228591	6737.720212	26.246119
205.456784	6730.690948	26.251136
205.473385	6736.553018	26.256154
205.233350	6746.325404	26.261172
205.977715	6762.637970	26.266189
206.225902	6766.998929	26.271207
206.222702	6766.085234	26.276224
206.354412	6794.914115	26.281242
206.666207	6791.164194	26.286260
206.705634	6796.769305	26.291277
206.967717	6821.758395	26.296295
207.259705	6823.504188	26.301312
207.224961	6836.058243	26.306330
207.424043	6843.719761	26.311348
207.906745	6847.052005	26.316365
208.107399	6857.237297	26.321383
208.582806	6869.173465	26.326400
208.207832	6882.336485	26.331418
208.902532	6889.337579	26.336436
208.769644	6910.837424	26.341453
208.860097	6913.913562	26.346471
209.327331	6924.752716	26.351488
209.419205	6950.193238	26.356506
209.728685	6948.737940	26.361524
210.121150	6957.629133	26.366541
210.216197	6973.360935	26.371559
210.594114	6967.516996	26.376576
210.571416	6986.338443	26.381594
210.779691	6997.243323	26.386612
211.081783	7000.856956	26.391629
211.251902	7008.276122	26.396647
211.676041	7009.639731	26.401664
211.876666	7039.493527	26.406682
211.968683	7040.203538	26.411700
212.249092	7033.764562	26.416717
212.247293	7047.891863	26.421735
212.566926	7050.678933	26.426752
212.590472	7061.958715	26.431770
212.771728	7058.637100	26.436788
213.130246	7076.067411	26.441805
213.018814	7099.381619	26.446823
213.936820	7083.157022	26.451840
213.668319	7090.673691	26.456858
213.975564	7106.105080	26.461876
214.345911	7112.975451	26.466893
214.356587	7121.687632	26.471911
214.596542	7117.702814	26.476928
214.565940	7131.335953	26.481946
214.837089	7145.066560	26.486964
215.259132	7145.946632	26.491981
214.985553	7164.831116	26.496999
215.124113	7172.261691	26.502016
215.700158	7181.328324	26.507034
215.398650	7199.618545	26.512052
215.873203	7206.761107	26.517069
216.209461	7234.638457	26.522087
216.365736	7238.524026	26.527104
216.610832	7253.728647	26.532122
216.535890	7268.339117	26.537140
217.003850	7273.216746	26.542157
217.049224	7288.206182	26.547175
217.616590	7317.792783	26.552192
218.100649	7321.578912	26.557210
218.302864	7320.840943	26.562228
218.496835	7335.046677	26.567245
218.632694	7350.254648	26.572263
219.102718	7348.337825	26.577280
219.181004	7355.147861	26.582298
219.145346	7367.858301	26.587316
219.835401	7373.404760	26.592333
219.781657	7379.188601	26.597351
220.264961	7396.390892	26.602368
220.578166	7397.913064	26.607386
220.344570	7407.695083	26.612404
220.582651	7400.437325	26.617421
220.910850	7420.927304	26.622439
221.362946	7427.797381	26.627456
221.241258	7428.632750	26.632474
221.406608	7446.977890	26.637492
222.185062	7449.793396	26.642509
222.006315	7450.030437	26.647527
222.422995	7446.810475	26.652544
222.592876	7468.101563	26.657562
222.648762	7488.010308	26.662580
222.924394	7485.166107	26.667597
222.772242	7496.600904	26.672615
223.307358	7511.334674	26.677632
223.199242	7514.898950	26.682650
223.069797	7534.841236	26.687668
223.653868	7539.159897	26.692685
223.966853	7564.323096	26.697703
224.298779	7575.502177	26.702720
224.707231	7574.953206	26.707738
224.880345	7591.349890	26.712756
225.155777	7598.625099	26.717773
225.022971	7613.847843	26.722791
225.421298	7613.928375	26.727808
225.509276	7628.128467	26.732826
225.456698	7629.690090	26.737844
226.050942	7622.289685	26.742861
226.145862	7646.815833	26.747879
226.337066	7659.103237	26.752896
226.864718	7668.003997	26.757914
226.665210	7673.937869	26.762932
227.047884	7684.256804	26.767949
227.101457	7705.220565	26.772967
227.755939	7713.234044	26.777984
227.980951	7723.345236	26.783002
228.067612	7728.508049	26.788020
228.510399	7744.617208	26.793037
228.476713	7745.753301	26.798055
228.678007	7750.114159	26.803072
229.240290	7761.735058	26.808090
229.075882	7781.920085	26.813108
229.475146	7779.374004	26.818125
229.599517	7797.292562	26.823143
229.857994	7810.653632	26.828160
230.267767	7816.712325	26.833178
230.137540	7836.603994	26.838196
230.673658	7841.284469	26.843213
230.978962	7842.554587	26.848231
230.855699	7869.058986	26.853248
231.260310	7869.456404	26.858266
231.349314	7883.334758	26.863284
231.692439	7884.931685	26.868301
232.145717	7896.199463	26.873319
232.240447	7909.985655	26.878336
232.589948	7914.189174	26.883354
232.702524	7929.137857	26.888372
233.046085	7941.116370	26.893389
233.072144	7953.500373	26.898407
233.258623	7957.021728	26.903424
233.615388	7972.294266	26.908442
233.771047	7984.503413	26.913460
233.755822	7984.642791	26.918477
233.931018	8011.392968	26.923495
234.172680	8020.817149	26.928512
234.996704	8027.049885	26.933530
234.825487	8040.374220	26.938548
235.269644	8053.217275	26.943565
235.703180	8069.893224	26.948583
235.821380	8075.099916	26.953600
236.127044	8077.068723	26.958618
236.261894	8088.931123	26.963636
236.603578	8091.505577	26.968653
236.704534	8095.863648	26.973671
236.862875	8108.919913	26.978688
237.332365	8116.498071	26.983706
237.021876	8131.154802	26.988724
237.519646	8142.480199	26.993741
237.722511	8145.710210	26.998759
237.749106	8151.152638	27.003776
238.159125	8163.007430	27.008794
238.168772	8187.998932	27.013812
238.529729	8180.998972	27.018829
238.552163	8206.235541	27.023847
238.537462	8212.937256	27.028864
239.075296	8229.784819	27.033882
239.162784	8253.327213	27.038900
239.542387	8265.903768	27.043917
239.853708	8281.387666	27.048935
240.203231	8294.172838	27.053952
240.810823	8299.758766	27.058970
240.802847	8303.628308	27.063988
241.544188	8310.126143	27.069005
241.153174	8332.733815	27.074023
241.538404	8330.662001	27.079040
242.078795	8326.488126	27.084058
242.373134	8345.640025	27.089076
242.561239	8349.171444	27.094093
242.809938	8350.412074	27.099111
243.081862	8356.929676	27.104128
243.379934	8374.108338	27.109146
243.350518	8374.900722	27.114164
243.739222	8379.837784	27.119181
244.069988	8389.174817	27.124199
244.198932	8409.998510	27.129216
244.584052	8405.655007	27.134234
244.328330	8410.881289	27.139252
244.913000	8431.607976	27.144269
245.220736	8428.018035	27.149287
245.121314	8435.550128	27.154304
245.503325	8450.637368	27.159322
245.667755	8467.973570	27.164340
246.051901	8465.111890	27.169357
246.038711	8481.786332	27.174375
245.905568	8502.395409	27.179392
246.578840	8518.874701	27.184410
246.761055	8535.019175	27.189428
247.126075	8551.330459	27.194445
247.228810	8550.553997	27.199463
247.429687	8566.629433	27.204480
247.748190	8578.619539	27.209498
247.808446	8601.737974	27.214516
247.913027	8622.691748	27.219533
248.101330	8633.293345	27.224551
248.313294	8648.514120	27.229568
249.088575	8664.971019	27.234586
249.198401	8682.884306	27.239604
249.435779	8691.487301	27.244621
249.613633	8706.887475	27.249639
249.907335	8714.768587	27.254656
250.080601	8726.084780	27.259674
250.845140	8745.342442	27.264692
250.650491	8752.443707	27.269709
251.009390	8763.332173	27.274727
250.916540	8769.484361	27.279744
251.545518	8781.987768	27.284762
251.603437	8801.292038	27.289780
251.941403	8815.694992	27.294797
252.404762	8813.024426	27.299815
252.432182	8829.487010	27.304832
252.836820	8832.397795	27.309850
252.735445	8852.691074	27.314868
253.034685	8855.872437	27.319885
253.428929	8876.988136	27.324903
253.694029	8898.785838	27.329920
253.918627	8898.557680	27.334938
254.124558	8915.576176	27.339956
254.481052	8927.669886	27.344973
254.693454	8934.886554	27.349991
254.934623	8963.514515	27.355008
255.864470	8951.873662	27.360026
255.674907	8959.842558	27.365044
255.924102	8976.312840	27.370061
256.305904	8983.181080	27.375079
256.171321	8996.146713	27.380096
256.767792	9015.018786	27.385114
256.678836	9015.265534	27.390132
256.874856	9030.138675	27.395149
257.701856	9039.443449	27.400167
257.299848	9056.561763	27.405184
257.944161	9069.181006	27.410202
257.894860	9062.079208	27.415220
257.713661	9111.331520	27.420237
258.745355	9081.540045	27.425255
258.465597	9142.766009	27.430272
259.235633	9125.565799	27.435290
259.275717	9148.597014	27.440308
259.432832	9172.140776	27.445325
259.743370	9172.943148	27.450343
259.853077	9191.052610	27.455360
260.221113	9216.344392	27.460378
260.710022	9231.423255	27.465396
260.668401	9228.626151	27.470413
261.158585	9241.775701	27.475431
261.050392	9262.579755	27.480448
261.685523	9283.008428	27.485466
261.789904	9296.924599	27.490484
262.199988	9319.838083	27.495501
262.872211	9315.963205	27.500519
263.129435	9338.686648	27.505536
263.653053	9337.987460	27.510554
263.685744	9344.015213	27.515572
264.401314	9340.703150	27.520589
264.241785	9343.620549	27.525607
264.447488	9368.370307	27.530624
264.941438	9370.930949	27.535642
264.952343	9378.079617	27.540660
264.654725	9380.495337	27.545677
265.151542	9382.391755	27.550695
265.190985	9407.624887	27.555712
265.732387	9418.013377	27.560730
265.731058	9417.942804	27.565748
265.718052	9441.696673	27.570765
265.969013	9445.711345	27.575783
266.144994	9472.571433	27.580800
266.792041	9473.757324	27.585818
266.458049	9500.615726	27.590836
266.897437	9512.268612	27.595853
267.278649	9534.798285	27.600871
267.631048	9550.699932	27.605888
268.276422	9558.112300	27.610906
268.118834	9587.516794	27.615924
268.694883	9599.396242	27.620941
268.982705	9602.762157	27.625959
269.054129	9628.603191	27.630976
269.435275	9637.751593	27.635994
269.463183	9649.802259	27.641012
269.748843	9666.258834	27.646029
270.174900	9678.501817	27.651047
270.553065	9698.305876	27.656064
270.755649	9715.531995	27.661082
271.409020	9735.381556	27.666100
271.079792	9742.740033	27.671117
271.623572	9743.431683	27.676135
271.881919	9768.161513	27.681152
272.261373	9778.661846	27.686170
272.621868	9800.715974	27.691188
272.549812	9806.004354	27.696205
273.396971	9820.489624	27.701223
273.575149	9825.639365	27.706240
274.055207	9838.263411	27.711258
273.917240	9861.235175	27.716276
273.964378	9874.814751	27.721293
274.409699	9888.555940	27.726311
274.544055	9907.364299	27.731328
274.709589	9920.635447	27.736346
275.147089	9935.191239	27.741364
275.364052	9963.760836	27.746381
275.951880	9959.070590	27.751399
276.059395	9980.523545	27.756416
276.177257	9987.527969	27.761434
276.487421	10011.037639	27.766452
276.972901	10028.955225	27.771469
277.549931	10012.423389	27.776487
277.738786	10041.882940	27.781504
277.815015	10055.546181	27.786522
277.942523	10060.203181	27.791540
278.353874	10076.371035	27.796557
278.485592	10085.690103	27.801575
278.279618	10097.622195	27.806592
278.757139	10121.476021	27.811610
278.896675	10143.482061	27.816628
279.211944	10161.720474	27.821645
280.161268	10166.219763	27.826663
280.072834	10177.916769	27.831680
280.439181	10198.499715	27.836698
280.975546	10212.939683	27.841716
280.784912	10228.609490	27.846733
281.212729	10240.696442	27.851751
281.649226	10255.581659	27.856768
281.573015	10259.797043	27.861786
282.045651	10272.672109	27.866804
282.172343	10288.385837	27.871821
282.863592	10302.452578	27.876839
282.675307	10318.239755	27.881856
282.837964	10340.792886	27.886874
283.522818	10353.516545	27.891892
283.623389	10370.783286	27.896909
284.078531	10378.283444	27.901927
284.134482	10399.369435	27.906944
284.492060	10408.723534	27.911962
284.635582	10423.474217	27.916980
285.106924	10445.687124	27.921997
285.190460	10453.193427	27.927015
285.729028	10474.139643	27.932032
285.594462	10498.074706	27.937050
286.411200	10498.678823	27.942068
286.791463	10521.511548	27.947085
286.920384	10526.494278	27.952103
287.088754	10557.574567	27.957120
287.329138	10571.545796	27.962138
287.472065	10578.615363	27.967156
287.625812	10603.638293	27.972173
288.273318	10617.788248	27.977191
288.278481	10638.547020	27.982208
288.645531	10659.328414	27.987226
289.286069	10677.910288	27.992244
289.390133	10687.438362	27.997261
289.602229	10703.793295	28.002279
289.666207	10722.537160	28.007296
290.279987	10744.867106	28.012314
290.794919	10756.270466	28.017332
290.696104	10767.737814	28.022349
291.292743	10764.524292	28.027367
291.701000	10801.394942	28.032384
291.929136	10813.081335	28.037402
292.563816	10823.389442	28.042420
292.414934	10838.337846	28.047437
292.894407	10843.369088	28.052455
292.903584	10869.089566	28.057472
293.406822	10877.372066	28.062490
294.159662	10886.539909	28.067508
294.232945	10908.362845	28.072525
294.362487	10906.283046	28.077543
294.955050	10926.445699	28.082560
294.732658	10937.452013	28.087578
295.177300	10941.293775	28.092596
295.310234	10962.291552	28.097613
295.358145	10971.033881	28.102631
295.508769	10978.722963	28.107648
295.878320	11000.655822	28.112666
296.104664	11001.574819	28.117684
296.404974	11016.783137	28.122701
296.591074	11028.381563	28.127719
296.916923	11053.966889	28.132736
296.809327	11077.505854	28.137754
297.361714	11095.993296	28.142772
297.600990	11123.939803	28.147789
298.064611	11140.751729	28.152807
298.300713	11167.376835	28.157824
298.758167	11186.174649	28.162842
299.443907	11206.274821	28.167860
299.498889	11214.119750	28.172877
300.010735	11238.844262	28.177895
300.337982	11252.510295	28.182912
300.439967	11266.430642	28.187930
300.788268	11281.323460	28.192948
300.922570	11295.350046	28.197965
301.483809	11300.452624	28.202983
301.580896	11329.155285	28.208000
301.823709	11345.622894	28.213018
302.447651	11358.780541	28.218036
302.483776	11385.384189	28.223053
302.619248	11406.230284	28.228071
303.151633	11419.482853	28.233088
303.333908	11439.346800	28.238106
303.835165	11459.281530	28.243124
304.192532	11482.536490	28.248141
304.527626	11495.372356	28.253159
304.745380	11506.875597	28.258176
305.158984	11516.084123	28.263194
305.588125	11523.838100	28.268212
305.861731	11548.869864	28.273229
306.077403	11559.851279	28.278247
306.651035	11574.427897	28.283264
306.815896	11598.601496	28.288282
307.139503	11587.138696	28.293300
307.211098	11622.574757	28.298317
307.582333	11632.192678	28.303335
307.833468	11643.429800	28.308352
307.927079	11662.685622	28.313370
308.572074	11678.343382	28.318388
308.793713	11695.013870	28.323405
309.266722	11717.294505	28.328423
309.495076	11721.338189	28.333440
309.777565	11751.328042	28.338458
309.880003	11760.892866	28.343476
310.087177	11777.399683	28.348493
310.616409	11780.755562	28.353511
310.737230	11801.729678	28.358528
310.768750	11827.954301	28.363546
311.682588	11846.087951	28.368564
311.633914	11863.767024	28.373581
312.069302	11881.719209	28.378599
312.164639	11894.684532	28.383616
312.182686	11910.651416	28.388634
312.674532	11930.176641	28.393652
312.893377	11969.496204	28.398669
313.375846	11982.374718	28.403687
313.718923	11991.740776	28.408704
313.694415	12019.427373	28.413722
314.176020	12020.124337	28.418740
314.632920	12041.076707	28.423757
315.003306	12061.830780	28.428775
315.490545	12069.948849	28.433792
315.594262	12100.894851	28.438810
315.866542	12109.566269	28.443828
316.537452	12133.872188	28.448845
316.859205	12151.021895	28.453863
317.467867	12164.130741	28.458880
317.321966	12186.791690	28.463898
317.786143	12197.963397	28.468916
317.975988	12216.206779	28.473933
318.360145	12240.650067	28.478951
318.686924	12246.510904	28.483968
318.902929	12270.517651	28.488986
319.175777	12288.155226	28.494004
319.390572	12304.182469	28.499021
319.820701	12319.100857	28.504039
320.155445	12346.027348	28.509056
320.203060	12369.958768	28.514074
320.541875	12375.995617	28.519092
321.473525	12391.788286	28.524109
321.777952	12415.576137	28.529127
322.078726	12430.176608	28.534144
322.057379	12444.483295	28.539162
322.818196	12466.363409	28.544180
322.784317	12475.117281	28.549197
323.236035	12499.062032	28.554215
323.755115	12508.066049	28.559232
323.759022	12531.964549	28.564250
324.143863	12535.766279	28.569268
324.719016	12557.979735	28.574285
324.823135	12576.059724	28.579303
325.313476	12588.124243	28.584320
325.493457	12609.060928	28.589338
325.753659	12616.430945	28.594356
326.224626	12639.450183	28.599373
326.414470	12656.488271	28.604391
327.032391	12674.043755	28.609408
326.904507	12675.526595	28.614426
327.700808	12701.358906	28.619444
328.006200	12715.119677	28.624461
328.126518	12729.521136	28.629479
328.435386	12744.150925	28.634496
328.541204	12767.024888	28.639514
329.147072	12777.090217	28.644532
329.343597	12799.963942	28.649549
329.470701	12801.632056	28.654567
330.018976	12815.523044	28.659584
330.116159	12847.801222	28.664602
330.357895	12863.530585	28.669620
330.556884	12874.086252	28.674637
330.506563	12886.889092	28.679655
331.261228	12910.803926	28.684672
331.784551	12940.425203	28.689690
331.946864	12950.105994	28.694708
331.941913	12981.291500	28.699725
332.426355	13008.471194	28.704743
332.959996	13022.466242	28.709760
333.306471	13047.627406	28.714778
333.814803	13063.160806	28.719796
334.013185	13079.551788	28.724813
334.236375	13089.034648	28.729831
334.678616	13117.584548	28.734848
334.840647	13135.060324	28.739866
334.952384	13167.382515	28.744884
335.501844	13181.968285	28.749901
336.170502	13203.710866	28.754919
336.127928	13223.181447	28.759936
336.568406	13253.185501	28.764954
337.033671	13259.136043	28.769972
337.110539	13296.433182	28.774989
337.311758	13325.714161	28.780007
337.879298	13341.147892	28.785024
338.000574	13374.974387	28.790042
338.558976	13394.440918	28.795060
339.089397	13412.128291	28.800077
339.487369	13441.510376	28.805095
339.883286	13458.055854	28.810112
340.108479	13479.246289	28.815130
340.628279	13492.172490	28.820148
341.119240	13521.799667	28.825165
341.223372	13534.973188	28.830183
341.944994	13547.693317	28.835200
342.528447	13566.045424	28.840218
342.713431	13574.532450	28.845236
342.939773	13587.853809	28.850253
342.909153	13606.388835	28.855271
343.678425	13627.922158	28.860288
344.018639	13634.389072	28.865306
344.249718	13654.036010	28.870324
344.700702	13655.893866	28.875341
344.849247	13687.687254	28.880359
345.361220	13695.321416	28.885376
345.361059	13711.888277	28.890394
345.513235	13730.818005	28.895412
346.118293	13750.825022	28.900429
345.979943	13773.044651	28.905447
346.669894	13790.836334	28.910464
346.760759	13816.756405	28.915482
347.072333	13839.629694	28.920500
347.807767	13851.108997	28.925517
348.041616	13882.523170	28.930535
348.375691	13890.945978	28.935552
348.138187	13914.894861	28.940570
348.764372	13927.457247	28.945588
349.274690	13953.576078	28.950605
349.327173	13971.381201	28.955623
350.172897	13986.366660	28.960640
350.236596	14015.405017	28.965658
350.685954	14038.169002	28.970676
351.279855	14048.117836	28.975693
351.439181	14069.726357	28.980711
351.761669	14094.490638	28.985728
352.296434	14117.953790	28.990746
352.210784	14132.727785	28.995764
352.600305	14136.932407	29.000781
352.853757	14170.571445	29.005799
353.625270	14201.075443	29.010816
353.858412	14211.487858	29.015834
353.976493	14236.681285	29.020852
354.926098	14248.963628	29.025869
354.879012	14275.263937	29.030887
355.336722	14306.262414	29.035904
355.597205	14314.528827	29.040922
356.074428	14340.514168	29.045940
356.050318	14363.912472	29.050957
356.501484	14390.106225	29.055975
356.930855	14403.911845	29.060992
357.224410	14427.123342	29.066010
357.724949	14455.839843	29.071028
358.306472	14478.456667	29.076045
358.346206	14506.993517	29.081063
359.033696	14520.024844	29.086080
359.170158	14541.925493	29.091098
359.485146	14571.948703	29.096116
360.226361	14595.642124	29.101133
360.302827	14621.302735	29.106151
360.969440	14636.526285	29.111168
361.073180	14665.050278	29.116186
361.180946	14687.473979	29.121204
361.950141	14701.930261	29.126221
362.162026	14722.479042	29.131239
362.591393	14737.548619	29.136256
363.076178	14760.709783	29.141274
363.447612	14780.095317	29.146292
364.060685	14802.818885	29.151309
364.024002	14818.263815	29.156327
364.547157	14832.393182	29.161344
365.055246	14852.169995	29.166362
365.124908	14872.189022	29.171380
365.574039	14891.696044	29.176397
366.185582	14904.479339	29.181415
366.552524	14928.230164	29.186432
366.660610	14947.722329	29.191450
367.161098	14965.527577	29.196468
367.669216	14971.773572	29.201485
367.536866	14987.326611	29.206503
367.907578	14999.233915	29.211520
368.120191	15012.559890	29.216538
368.626559	15034.966045	29.221556
369.144569	15052.010611	29.226573
369.366594	15071.945300	29.231591
369.871149	15089.741287	29.236608
370.053946	15122.470962	29.241626
370.243364	15140.258675	29.246644
370.706209	15142.697869	29.251661
370.762565	15180.426697	29.256679
371.151400	15198.032734	29.261696
371.392288	15215.170450	29.266714
371.432459	15257.784516	29.271732
371.932725	15288.229707	29.276749
372.283077	15319.958218	29.281767
372.927789	15354.958565	29.286784
373.191845	15379.960671	29.291802
373.630725	15410.134351	29.296820
374.451133	15431.809203	29.301837
374.547578	15477.543881	29.306855
375.414442	15476.713411	29.311872
375.744514	15499.904582	29.316890
376.058696	15533.668410	29.321908
376.675479	15555.774426	29.326925
376.926869	15577.885560	29.331943
377.602261	15593.444136	29.336960
378.099325	15607.909812	29.341978
378.209876	15629.821459	29.346996
378.834622	15642.333738	29.352013
378.901506	15660.436208	29.357031
379.241220	15676.397896	29.362048
379.800426	15696.152726	29.367066
379.882705	15714.254282	29.372084
380.383059	15734.797426	29.377101
380.479636	15755.789313	29.382119
381.259894	15780.668291	29.387136
381.396064	15799.367841	29.392154
381.634771	15828.434396	29.397172
382.082365	15847.905687	29.402189
382.302348	15880.790374	29.407207
382.569407	15907.413435	29.412224
383.250530	15931.519817	29.417242
383.295398	15964.571047	29.422260
384.008407	15980.883734	29.427277
384.284805	16010.547770	29.432295
384.900793	16024.100360	29.437312
385.327440	16044.636278	29.442330
385.571019	16072.471822	29.447348
386.319869	16094.652834	29.452365
386.499360	16111.560825	29.457383
387.038283	16133.861256	29.462400
387.624305	16151.095197	29.467418
388.082301	16163.433426	29.472436
388.337691	16169.696866	29.477453
388.566130	16209.432261	29.482471
389.021921	16194.423874	29.487488
389.164814	16221.365739	29.492506
389.323541	16237.820754	29.497524
389.849295	16254.311384	29.502541
389.770330	16269.970776	29.507559
389.700104	16301.854246	29.512576
390.536261	16328.061913	29.517594
390.762330	16354.207019	29.522612
390.858181	16375.083742	29.527629
391.459445	16414.676219	29.532647
392.019954	16439.905905	29.537664
392.634782	16472.459986	29.542682
393.117129	16503.176845	29.547700
393.891233	16495.757518	29.552717
393.703867	16557.797107	29.557735
394.105775	16566.754315	29.562752
394.619132	16588.553841	29.567770
395.305061	16615.300238	29.572788
395.748532	16648.458691	29.577805
396.051516	16663.666140	29.582823
396.015699	16682.698164	29.587840
396.699193	16707.006644	29.592858
396.625203	16753.182747	29.597876
397.506045	16759.639845	29.602893
397.832281	16778.909932	29.607911
398.025268	16813.456518	29.612928
398.664747	16847.994040	29.617946
398.904223	16880.858764	29.622964
399.780794	16902.404823	29.627981
399.751534	16918.868080	29.632999
400.330651	16946.654792	29.638016
401.345264	16959.189392	29.643034
401.424324	17003.065337	29.648052
402.141307	17009.829330	29.653069
402.565102	17022.498077	29.658087
402.917328	17055.206246	29.663104
403.320795	17065.529104	29.668122
403.874742	17089.732468	29.673140
404.307704	17100.799589	29.678157
404.023459	17118.068175	29.683175
404.781761	17137.145668	29.688192
404.986943	17161.827901	29.693210
405.247164	17192.747262	29.698228
405.591530	17201.769517	29.703245
405.913319	17231.494022	29.708263
406.322536	17262.587401	29.713280
406.617736	17257.702855	29.718298
407.093178	17307.560247	29.723316
407.832749	17330.488066	29.728333
407.981421	17351.166176	29.733351
408.112239	17376.793986	29.738368
409.165382	17391.208866	29.743386
409.630384	17416.379593	29.748404
410.143442	17406.803778	29.753421
410.518574	17446.586896	29.758439
410.813813	17451.480644	29.763456
411.471773	17460.573353	29.768474
411.577384	17474.057087	29.773492
412.141539	17497.582353	29.778509
412.189102	17511.838696	29.783527
412.599239	17529.290191	29.788544
413.159017	17542.264645	29.793562
413.292409	17568.912368	29.798580
413.685654	17589.862831	29.803597
414.385993	17605.985194	29.808615
414.630715	17638.316481	29.813632
415.020807	17656.682671	29.818650
415.317249	17685.555649	29.823668
415.601038	17709.043631	29.828685
415.936799	17749.565450	29.833703
416.509541	17777.300941	29.838720
417.021760	17781.317556	29.843738
416.972807	17823.930473	29.848756
417.186043	17846.265008	29.853773
417.909301	17862.073769	29.858791
418.021856	17911.706101	29.863808
418.774618	17941.761515	29.868826
419.157624	17977.023305	29.873844
419.865501	18001.417346	29.878861
420.105525	18033.518327	29.883879
420.257828	18060.996525	29.888896
421.305828	18099.321414	29.893914
421.319147	18127.400593	29.898932
421.799280	18156.730205	29.903949
422.339020	18185.391342	29.908967
422.802930	18219.659723	29.913984
423.321167	18233.016172	29.919002
423.604206	18266.264291	29.924020
424.094703	18299.552654	29.929037
424.729198	18335.705484	29.934055
424.567508	18361.245703	29.939072
424.863025	18385.416687	29.944090
425.408863	18413.454845	29.949108
425.601855	18455.432136	29.954125
426.537583	18476.046191	29.959143
427.079481	18502.697362	29.964160
427.548697	18532.637293	29.969178
427.973274	18570.041426	29.974196
428.421256	18596.545124	29.979213
428.698466	18627.591808	29.984231
429.208761	18656.702995	29.989248
430.008696	18675.561397	29.994266
430.198733	18709.747724	29.999284
430.250624	18738.334854	30.004301
430.908155	18762.967648	30.009319
431.211841	18796.889208	30.014336
431.769145	18816.194315	30.019354
432.011908	18850.322157	30.024372
432.379614	18873.215456	30.029389
433.098537	18894.496905	30.034407
433.282254	18922.300761	30.039424
434.175302	18937.666248	30.044442
434.188363	18957.543289	30.049460
434.514269	18982.374546	30.054477
434.881643	19004.553511	30.059495
435.176169	19046.229601	30.064512
436.003785	19066.189214	30.069530
436.130732	19103.871585	30.074548
436.774129	19140.141805	30.079565
437.010032	19166.257024	30.084583
437.057616	19203.831805	30.089600
437.637562	19229.399387	30.094618
438.206634	19261.620565	30.099636
438.568824	19294.127143	30.104653
438.907627	19330.138054	30.109671
439.432338	19366.947813	30.114688
439.982789	19401.605033	30.119706
440.273354	19449.302010	30.124724
440.840047	19472.865312	30.129741
441.554867	19504.122780	30.134759
441.834965	19546.805710	30.139776
442.452330	19577.120530	30.144794
442.878737	19611.831447	30.149812
443.186672	19636.906390	30.154829
443.680026	19669.668855	30.159847
444.314423	19708.581767	30.164864
444.748001	19721.384056	30.169882
445.080606	19764.356086	30.174900
445.711858	19798.218191	30.179917
446.187607	19829.422268	30.184935
446.461073	19864.975892	30.189952
446.977092	19889.212123	30.194970
447.397189	19907.714400	30.199988
448.035588	19949.190076	30.205005
448.439254	19975.397255	30.210023
448.764123	20000.630334	30.215040
449.405745	20022.493020	30.220058
449.709390	20055.322350	30.225076
449.919310	20098.735355	30.230093
450.905270	20111.069614	30.235111
451.083181	20152.625493	30.240128
451.481277	20179.919439	30.245146
452.024482	20212.125838	30.250164
452.271399	20244.936648	30.255181
452.982836	20278.963419	30.260199
453.249107	20307.017247	30.265216
453.534358	20334.566868	30.270234
453.863720	20362.837540	30.275252
454.535061	20403.585475	30.280269
455.396965	20439.342755	30.285287
455.721739	20475.802296	30.290304
456.153583	20496.204407	30.295322
456.554651	20517.791115	30.300340
456.786644	20560.945162	30.305357
457.664689	20552.618507	30.310375
457.709206	20605.912422	30.315392
458.011130	20611.901327	30.320410
458.468337	20635.649995	30.325428
458.541341	20671.577982	30.330445
459.013745	20704.240827	30.335463
459.474900	20744.122624	30.340480
460.204328	20781.661869	30.345498
460.706941	20822.611423	30.350516
460.808080	20852.763686	30.355533
461.785432	20877.040965	30.360551
462.188752	20919.810388	30.365568
462.675452	20954.172508	30.370586
463.164613	20988.494935	30.375604
463.692906	21013.892940	30.380621
464.209691	21050.589411	30.385639
464.441558	21087.815684	30.390656
464.825012	21114.020117	30.395674
465.160344	21135.749667	30.400692
465.381869	21181.279115	30.405709
466.288367	21217.148414	30.410727
466.538585	21257.286811	30.415744
467.067860	21292.274489	30.420762
467.987751	21321.381712	30.425780
468.284705	21365.648285	30.430797
468.931137	21395.118161	30.435815
469.148428	21428.647710	30.440832
469.737177	21460.759645	30.445850
470.464856	21489.985219	30.450868
470.691764	21513.859719	30.455885
471.426752	21549.217635	30.460903
471.778169	21593.284011	30.465920
472.326927	21623.357388	30.470938
472.662232	21647.614898	30.475956
473.324447	21682.688589	30.480973
473.908939	21706.539494	30.485991
474.005640	21734.835923	30.491008
474.209677	21766.348225	30.496026
474.983426	21804.434151	30.501044
475.219096	21842.074285	30.506061
475.701280	21887.043673	30.511079
476.258574	21917.722677	30.516096
476.734506	21952.515558	30.521114
477.533817	21996.120291	30.526132
477.896422	22028.178055	30.531149
478.181794	22056.861631	30.536167
478.996140	22099.813723	30.541184
479.326364	22123.199358	30.546202
479.891547	22161.606052	30.551220
480.190045	22198.665249	30.556237
480.821002	22220.963518	30.561255
481.043077	22270.619007	30.566272
481.567090	22292.789499	30.571290
482.203035	22309.997739	30.576308
482.838001	22342.207288	30.581325
483.278426	22373.094820	30.586343
483.505172	22382.508997	30.591360
483.786536	22430.799319	30.596378
484.770655	22457.379711	30.601396
484.979429	22476.829936	30.606413
485.198021	22510.889268	30.611431
485.825369	22543.608441	30.616448
486.596256	22582.454376	30.621466
486.585525	22610.139411	30.626484
487.021530	22652.657882	30.631501
487.608705	22677.455744	30.636519
488.173309	22708.197346	30.641536
488.652495	22757.788994	30.646554
489.234679	22780.331321	30.651572
489.660489	22817.425247	30.656589
490.166339	22846.283066	30.661607
490.177763	22888.317692	30.666624
490.863436	22930.994832	30.671642
491.135950	22970.606339	30.676660
491.511129	23016.848306	30.681677
492.223563	23041.105382	30.686695
493.123089	23091.521916	30.691712
493.546842	23137.895121	30.696730
494.196680	23173.464009	30.701748
494.706822	23199.533592	30.706765
495.443816	23234.524792	30.711783
495.647365	23275.434247	30.716800
496.466099	23305.770283	30.721818
496.942187	23336.761138	30.726836
497.100478	23379.896840	30.731853
498.010253	23408.693706	30.736871
498.407758	23442.029483	30.741888
498.620854	23485.685248	30.746906
499.460535	23516.259371	30.751924
499.593397	23557.381663	30.756941
500.293147	23577.581273	30.761959
500.775484	23624.930343	30.766976
500.925272	23660.069585	30.771994
501.831440	23699.289758	30.777012
502.219863	23734.117048	30.782029
502.790848	23767.580255	30.787047
503.203663	23801.089208	30.792064
503.644330	23837.865734	30.797082
504.369234	23872.824829	30.802100
504.612940	23920.497928	30.807117
505.130225	23954.242615	30.812135
505.573909	23988.914368	30.817152
506.114685	24025.164973	30.822170
506.901592	24065.736213	30.827188
507.078976	24103.313032	30.832205
507.769533	24133.817584	30.837223
508.437117	24159.815622	30.842240
508.532514	24201.194453	30.847258
509.145885	24234.379359	30.852276
509.608619	24264.788123	30.857293
510.317871	24294.023414	30.862311
510.784247	24331.208158	30.867328
511.140093	24358.912680	30.872346
512.247686	24381.835975	30.877364
512.412227	24416.765015	30.882381
513.229070	24435.387449	30.887399
513.181504	24468.500894	30.892416
513.852863	24502.339572	30.897434
514.771848	24535.800169	30.902452
515.045932	24565.744100	30.907469
515.662665	24596.342435	30.912487
515.982478	24629.507974	30.917504
516.246347	24662.643895	30.922522
516.922324	24688.281485	30.927540
517.609889	24725.862006	30.932557
517.961117	24761.820740	30.937575
518.236969	24794.013718	30.942592
518.824719	24826.765978	30.947610
519.491080	24863.307275	30.952628
519.658669	24912.069117	30.957645
520.038271	24949.288821	30.962663
520.552683	24998.544721	30.967680
521.069530	25033.054281	30.972698
521.811168	25071.079154	30.977716
522.128373	25125.426389	30.982733
522.693770	25165.038464	30.987751
523.124108	25212.656556	30.992768
523.784937	25244.096709	30.997786
524.397619	25295.647496	31.002804
524.841539	25344.816438	31.007821
525.568425	25381.877066	31.012839
526.339468	25419.634985	31.017856
526.768095	25466.177268	31.022874
527.505033	25496.628211	31.027892
528.033220	25531.206365	31.032909
528.819209	25554.944337	31.037927
529.593045	25603.247786	31.042944
529.926218	25630.975463	31.047962
530.665418	25643.278981	31.052980
531.068509	25687.978707	31.057997
531.716608	25712.960681	31.063015
531.875442	25741.830989	31.068032
532.257511	25790.120205	31.073050
532.860460	25812.235792	31.078068
533.543591	25849.294236	31.083085
533.802893	25883.265292	31.088103
534.342118	25913.450751	31.093120
534.810574	25952.539818	31.098138
535.433452	25985.039143	31.103156
535.589045	26031.120027	31.108173
536.440177	26071.760993	31.113191
537.553014	26104.284144	31.118208
537.550882	26141.068768	31.123226
538.455968	26151.604493	31.128244
538.859842	26187.781780	31.133261
539.280369	26236.832724	31.138279
540.082448	26233.839861	31.143296
540.179713	26273.664748	31.148314
540.895167	26293.766063	31.153332
541.152034	26344.971201	31.158349
541.603158	26371.029393	31.163367
542.111003	26397.188095	31.168384
542.374099	26438.958020	31.173402
543.046054	26465.988774	31.178420
543.268964	26526.859776	31.183437
543.647210	26561.329328	31.188455
544.404573	26595.401393	31.193472
544.896444	26655.613988	31.198490
545.506139	26693.414011	31.203508
546.119568	26751.374189	31.208525
546.736454	26795.495430	31.213543
547.503488	26824.776587	31.218560
547.894319	26870.928767	31.223578
548.740286	26906.004443	31.228596
549.248858	26954.460577	31.233613
549.588473	26993.405687	31.238631
550.619613	27023.278546	31.243648
550.918794	27078.012638	31.248666
551.684186	27109.820327	31.253684
552.057899	27146.281104	31.258701
552.522723	27186.060738	31.263719
553.235859	27224.534097	31.268736
553.469232	27267.124732	31.273754
554.170042	27305.842899	31.278772
554.866144	27338.176530	31.283789
555.621298	27383.074650	31.288807
556.358338	27408.712405	31.293824
556.996679	27453.596238	31.298842
557.583907	27476.355569	31.303860
557.834821	27514.510109	31.308877
558.389822	27556.602002	31.313895
559.220990	27587.162462	31.318912
559.558660	27621.722687	31.323930
560.142628	27659.274608	31.328948
560.638920	27694.448670	31.333965
561.194273	27727.420025	31.338983
561.800017	27761.494294	31.344000
562.458038	27806.106530	31.349018
562.840982	27832.320556	31.354036
563.305446	27887.461241	31.359053
563.572479	27914.733835	31.364071
564.586633	27955.764880	31.369088
564.711544	28000.451530	31.374106
565.481664	28036.288653	31.379124
566.231774	28082.779442	31.384141
566.516185	28131.678208	31.389159
567.409995	28159.612474	31.394176
567.940189	28201.245946	31.399194
568.278031	28242.959008	31.404212
568.987078	28274.239859	31.409229
569.497592	28306.360754	31.414247
570.277685	28325.902026	31.419264
570.569229	28371.384133	31.424282
570.996576	28405.354236	31.429300
571.774392	28438.195494	31.434317
571.913096	28469.373739	31.439335
572.689520	28512.938516	31.444352
573.264110	28546.352853	31.449370
573.592906	28589.499059	31.454388
574.588117	28632.307605	31.459405
574.837596	28665.313834	31.464423
575.644237	28695.089259	31.469440
575.955929	28756.785765	31.474458
576.998373	28772.317929	31.479476
577.575939	28809.859366	31.484493
577.697889	28867.662754	31.489511
578.770127	28908.155926	31.494528
578.662861	28948.097989	31.499546
579.653650	28996.437759	31.504564
579.993845	29034.636821	31.509581
580.590266	29071.909549	31.514599
581.435271	29111.237059	31.519616
581.748529	29173.043631	31.524634
582.189753	29216.785029	31.529652
583.206444	29251.742505	31.534669
583.733864	29291.535481	31.539687
584.320466	29336.336660	31.544704
584.825204	29383.453336	31.549722
585.129312	29422.250006	31.554740
586.026135	29476.559801	31.559757
586.342566	29523.741543	31.564775
587.195117	29562.761652	31.569792
587.730459	29622.545804	31.574810
588.366322	29657.906776	31.579828
589.143082	29696.201761	31.584845
589.722771	29751.516397	31.589863
590.540963	29773.771785	31.594880
591.140400	29826.227999	31.599898
591.782712	29856.762955	31.604916
592.221299	29903.325922	31.609933
592.446027	29941.922150	31.614951
593.266316	29972.094885	31.619968
593.851862	30032.091601	31.624986
594.162854	30077.709345	31.630004
594.635543	30125.490438	31.635021
595.300764	30172.987284	31.640039
596.114019	30224.912734	31.645056
596.227726	30271.878353	31.650074
597.313371	30318.121979	31.655092
598.001189	30347.389848	31.660109
598.709847	30402.881577	31.665127
599.365603	30441.389857	31.670144
600.135785	30492.213541	31.675162
600.682575	30521.214204	31.680180
601.323621	30550.053342	31.685197
601.762950	30585.707668	31.690215
602.691546	30603.127272	31.695232
602.902515	30644.154363	31.700250
603.430718	30674.281936	31.705268
604.192580	30709.467531	31.710285
604.299375	30747.242866	31.715303
604.961948	30793.911396	31.720320
605.391552	30822.185809	31.725338
605.930159	30879.606900	31.730356
606.674336	30913.326914	31.735373
607.115972	30966.420268	31.740391
607.762522	31004.187465	31.745408
608.428700	31055.261142	31.750426
609.088821	31098.301349	31.755444
609.986928	31144.780498	31.760461
610.503212	31196.702753	31.765479
610.866522	31239.365068	31.770496
611.383811	31284.850888	31.775514
611.910607	31324.543336	31.780532
612.673293	31375.776011	31.785549
613.170299	31433.558708	31.790567
613.863915	31476.310885	31.795584
614.525027	31531.421581	31.800602
614.997689	31581.824791	31.805620
615.932493	31624.422318	31.810637
616.196058	31682.955456	31.815655
616.901252	31727.868835	31.820672
617.712330	31779.619905	31.825690
618.249316	31833.432193	31.830708
619.157239	31876.208027	31.835725
619.690548	31931.912547	31.840743
620.058904	31978.040266	31.845760
620.513617	32026.156033	31.850778
621.508726	32069.687634	31.855796
622.473210	32128.884619	31.860813
622.747989	32187.668373	31.865831
623.655555	32224.886156	31.870848
624.289985	32270.078656	31.875866
624.598106	32328.778797	31.880884
625.627383	32362.409117	31.885901
626.130248	32404.015130	31.890919
626.573322	32456.271413	31.895936
627.326260	32506.423200	31.900954
627.875606	32557.562719	31.905972
628.801121	32595.932242	31.910989
629.073040	32646.772611	31.916007
629.759098	32685.122155	31.921024
630.498468	32730.031259	31.926042
631.012780	32785.074968	31.931060
632.031599	32813.720817	31.936077
632.454492	32867.066037	31.941095
633.303172	32918.581433	31.946112
633.789207	32959.906240	31.951130
634.024842	32988.248378	31.956148
634.982340	33028.659740	31.961165
635.404412	33080.804708	31.966183
636.028226	33111.422777	31.971200
636.858290	33146.899084	31.976218
637.467099	33194.114194	31.981236
638.068706	33223.952623	31.986253
638.514267	33273.737995	31.991271
639.601195	33312.446024	31.996288
640.136518	33348.013833	32.001306
640.488171	33383.874199	32.006324
641.166875	33412.551610	32.011341
641.386581	33469.971062	32.016359
642.233356	33524.466203	32.021376
642.965489	33555.851252	32.026394
643.306130	33612.099692	32.031412
643.997416	33667.248995	32.036429
644.339451	33726.311250	32.041447
645.069061	33776.298805	32.046464
645.765217	33837.617478	32.051482
646.328799	33888.227646	32.056500
647.584751	33945.266213	32.061517
647.811959	33993.800684	32.066535
648.542314	34036.541059	32.071552
649.461468	34087.240237	32.076570
649.852443	34134.913598	32.081588
650.477241	34198.595262	32.086605
651.161660	34245.760353	32.091623
651.728870	34292.141889	32.096640
652.588846	34348.887073	32.101658
653.165294	34402.193879	32.106676
654.087203	34447.540461	32.111693
654.560738	34507.930762	32.116711
655.190081	34556.153782	32.121728
656.304598	34606.180289	32.126746
656.657039	34655.681982	32.131764
657.353831	34709.985795	32.136781
657.967695	34765.690203	32.141799
658.390985	34808.733685	32.146816
659.137313	34858.124394	32.151834
659.447368	34939.872399	32.156852
660.484339	34978.272284	32.161869
660.926491	35039.500275	32.166887
661.413384	35100.607866	32.171904
662.624293	35144.926660	32.176922
662.923262	35196.735312	32.181940
663.646681	35258.732756	32.186957
664.531054	35313.089070	32.191975
665.213285	35363.687998	32.196992
666.079123	35419.077021	32.202010
666.411130	35482.357785	32.207028
667.840958	35516.175118	32.212045
668.192664	35571.764746	32.217063
668.711246	35605.820365	32.222080
669.605466	35666.226709	32.227098
670.274155	35699.244953	32.232116
670.750875	35732.762040	32.237133
671.351344	35771.952134	32.242151
671.712382	35828.182755	32.247168
672.918773	35867.193043	32.252186
672.941774	35918.838205	32.257204
673.856668	35952.889763	32.262221
674.394125	36022.365423	32.267239
674.818458	36068.837722	32.272256
675.526049	36115.550397	32.277274
675.967215	36168.515497	32.282292
676.583661	36219.220511	32.287309
677.427369	36283.652519	32.292327
678.040748	36353.781182	32.297344
678.853290	36401.464853	32.302362
679.242287	36462.126362	32.307380
680.354956	36515.280457	32.312397
680.837090	36575.106167	32.317415
681.309653	36634.671906	32.322432
682.592820	36687.927104	32.327450
682.788381	36740.220513	32.332468
683.572186	36814.266957	32.337485
684.221692	36871.542986	32.342503
685.214085	36917.501521	32.347520
685.814661	36975.096281	32.352538
686.124779	37050.712215	32.357556
687.019571	37103.062543	32.362573
687.479531	37166.994627	32.367591
688.207380	37212.658698	32.372608
689.113437	37279.958769	32.377626
689.767315	37342.960401	32.382644
690.582225	37399.480346	32.387661
691.071093	37468.856218	32.392679
691.899648	37529.327045	32.397696
692.984001	37582.487461	32.402714
693.426381	37641.095093	32.407732
694.311278	37697.444080	32.412749
695.168322	37761.545394	32.417767
695.748484	37819.379644	32.422784
696.491103	37875.966308	32.427802
696.912844	37930.177746	32.432820
697.545024	37992.893581	32.437837
698.556261	38052.304477	32.442855
699.199349	38114.505029	32.447872
699.883942	38165.510953	32.452890
700.528824	38229.926904	32.457908
701.418800	38281.118064	32.462925
702.184600	38339.555227	32.467943
702.644645	38400.986583	32.472960
703.402886	38456.120550	32.477978
704.130853	38500.517260	32.482996
704.695519	38569.590747	32.488013
705.328323	38640.038046	32.493031
705.656036	38690.307696	32.498048
707.188539	38745.227888	32.503066
707.247290	38810.420527	32.508084
708.223893	38858.430365	32.513101
708.626858	38920.230621	32.518119
709.170228	38971.141628	32.523136
709.963639	39024.740806	32.528154
710.831390	39090.018587	32.533172
711.516286	39138.203382	32.538189
712.184081	39190.151688	32.543207
712.876281	39261.743178	32.548224
713.468106	39309.421357	32.553242
714.192109	39374.685279	32.558260
714.721446	39428.435000	32.563277
715.565913	39490.887652	32.568295
716.165690	39558.537289	32.573312
717.179392	39619.369299	32.578330
717.750430	39677.651296	32.583348
718.698478	39735.819860	32.588365
719.578947	39801.615563	32.593383
720.196096	39861.437740	32.598400
720.781940	39917.001280	32.603418
721.566282	39985.686040	32.608436
722.316006	40050.210492	32.613453
723.377904	40105.793474	32.618471
723.819180	40176.094729	32.623488
724.259611	40225.523118	32.628506
725.083807	40295.402797	32.633524
726.168718	40350.620231	32.638541
726.881310	40414.825559	32.643559
727.419610	40479.697526	32.648576
728.363262	40537.252962	32.653594
728.880156	40600.102455	32.658612
729.529636	40665.173466	32.663629
730.614058	40731.038067	32.668647
731.269044	40791.474072	32.673664
732.076892	40848.035051	32.678682
732.515206	40914.257108	32.683700
733.763809	40965.290478	32.688717
734.046267	41037.473492	32.693735
734.799377	41098.215085	32.698752
736.063249	41158.153328	32.703770
736.381645	41232.520285	32.708788
736.965529	41289.943145	32.713805
738.228592	41347.447315	32.718823
738.511440	41404.284532	32.723840
739.675008	41464.839081	32.728858
740.148751	41532.820982	32.733876
741.116219	41591.372856	32.738893
741.660297	41640.202193	32.743911
742.399184	41709.022561	32.748928
743.305767	41765.058327	32.753946
743.780652	41837.488483	32.758964
744.575514	41899.077875	32.763981
745.747732	41958.923128	32.768999
746.071124	42017.143725	32.774016
746.989700	42074.746188	32.779034
747.368692	42125.060389	32.784052
748.040874	42170.659944	32.789069
749.116832	42226.203445	32.794087
749.219517	42293.824776	32.799104
750.178697	42345.343622	32.804122
750.728024	42405.980359	32.809140
751.588173	42475.828534	32.814157
752.508253	42531.214894	32.819175
753.255408	42602.384257	32.824192
753.992606	42665.253574	32.829210
754.617919	42716.668972	32.834228
755.284072	42785.006864	32.839245
755.892270	42843.894628	32.844263
756.493762	42920.337182	32.849280
757.271083	42995.086621	32.854298
757.992391	43058.675927	32.859316
758.690668	43135.006242	32.864333
759.948348	43208.390027	32.869351
760.753304	43283.164706	32.874368
761.526873	43347.633129	32.879386
761.818542	43412.124879	32.884404
762.699635	43482.374409	32.889421
763.595658	43553.404136	32.894439
764.031009	43637.841148	32.899456
765.170146	43703.763668	32.904474
765.736724	43770.380078	32.909492
766.343830	43840.854482	32.914509
767.727425	43911.968948	32.919527
768.401188	43988.587684	32.924544
769.407534	44045.211197	32.929562
770.007172	44122.104145	32.934580
771.020517	44192.770832	32.939597
772.161947	44250.389265	32.944615
772.196968	44323.294194	32.949632
773.343907	44389.823761	32.954650
774.133575	44450.956232	32.959668
774.892563	44536.415500	32.964685
775.896445	44591.927633	32.969703
776.484017	44656.367450	32.974720
777.298350	44710.944833	32.979738
778.271614	44791.942195	32.984756
778.963080	44847.987535	32.989773
779.853908	44909.831086	32.994791
780.526620	44977.063011	32.999808
781.068555	45044.186673	33.004826
782.033770	45100.482636	33.009844
782.779166	45179.521172	33.014861
783.595239	45235.219839	33.019879
784.063715	45302.832550	33.024896
785.078552	45376.339903	33.029914
785.648521	45439.195446	33.034932
786.668887	45510.503638	33.039949
787.712957	45570.539564	33.044967
788.445264	45639.906644	33.049984
789.116036	45702.762866	33.055002
789.992542	45751.935798	33.060020
790.696002	45820.696160	33.065037
791.310672	45870.049914	33.070055
791.982145	45935.563213	33.075072
792.835512	45989.037364	33.080090
793.506040	46052.298703	33.085108
794.233224	46111.008266	33.090125
795.280023	46165.774053	33.095143
795.639067	46233.000810	33.100160
796.281172	46308.562149	33.105178
797.313128	46373.527551	33.110196
797.805017	46453.782678	33.115213
798.925663	46522.331119	33.120231
799.399486	46594.251298	33.125248
800.411292	46658.996967	33.130266
801.249313	46732.115415	33.135284
802.096426	46793.931597	33.140301
802.900119	46856.266016	33.145319
803.845062	46938.609264	33.150336
804.388376	47007.500743	33.155354
805.417995	47076.110011	33.160372
805.747838	47169.153133	33.165389
807.069033	47232.018598	33.170407
807.580616	47308.362236	33.175424
807.901117	47368.765606	33.180442
809.102376	47458.191508	33.185460
809.610419	47553.461036	33.190477
810.861109	47607.432193	33.195495
811.590330	47697.701139	33.200512
812.295497	47773.921331	33.205530
813.487587	47850.206335	33.210548
814.505330	47927.071575	33.215565
815.364453	47995.465470	33.220583
815.891306	48077.060247	33.225600
816.983864	48130.521797	33.230618
817.799044	48215.018293	33.235636
818.249793	48287.526478	33.240653
819.545846	48360.354777	33.245671
820.146439	48439.882270	33.250688
821.005938	48513.926049	33.255706
821.909571	48577.774667	33.260724
822.385983	48659.465357	33.265741
823.376314	48739.790412	33.270759
824.002622	48813.645379	33.275776
824.665653	48888.529763	33.280794
825.414187	48960.753507	33.285812
826.240272	49044.829417	33.290829
827.593403	49127.392450	33.295847
827.983488	49214.264815	33.300864
828.779551	49290.884135	33.305882
829.684012	49353.564762	33.310900
830.390201	49456.733149	33.315917
831.475834	49539.359610	33.320935
832.656195	49599.204610	33.325952
833.184683	49695.687817	33.330970
834.153005	49756.520053	33.335988
835.010897	49831.917001	33.341005
835.555955	49894.688297	33.346023
836.629813	49954.570380	33.351040
837.357634	50029.954159	33.356058
838.126667	50098.342122	33.361076
838.981749	50173.113007	33.366093
839.842628	50237.876910	33.371111
840.239915	50313.901436	33.376128
841.157888	50389.502611	33.381146
842.067383	50464.408063	33.386164
842.689443	50548.545652	33.391181
844.174857	50615.761294	33.396199
844.563448	50691.432224	33.401216
845.598847	50769.045418	33.406234
846.544686	50851.769652	33.411252
847.010506	50926.255367	33.416269
848.147558	51017.445112	33.421287
849.054002	51094.587951	33.426304
849.822933	51170.635872	33.431322
851.013029	51245.566219	33.436340
851.496934	51321.016364	33.441357
852.504016	51397.267187	33.446375
853.538614	51481.125763	33.451392
854.180972	51559.243600	33.456410
855.151221	51630.960054	33.461428
855.780479	51717.850732	33.466445
856.716261	51796.219554	33.471463
857.601749	51873.173422	33.476480
858.262769	51968.641091	33.481498
859.520363	52040.001020	33.486516
860.118134	52125.345976	33.491533
861.094326	52200.453224	33.496551
861.762261	52279.311769	33.501568
862.755332	52375.688165	33.506586
863.927887	52441.650748	33.511604
864.775270	52541.917293	33.516621
865.620767	52625.334758	33.521639
866.374673	52692.270659	33.526656
867.185374	52768.044132	33.531674
868.217402	52847.361659	33.536692
868.863759	52942.953605	33.541709
869.657065	53025.393381	33.546727
870.727367	53112.062803	33.551744
871.476262	53197.729649	33.556762
872.360148	53278.508679	33.561780
873.365332	53372.685509	33.566797
873.953136	53444.896142	33.571815
874.982614	53529.396321	33.576832
875.851311	53620.903956	33.581850
877.239918	53698.606172	33.586868
877.431055	53787.710143	33.591885
878.175409	53871.695489	33.596903
879.633190	53954.311510	33.601920
880.271536	54037.490717	33.606938
881.269063	54113.792450	33.611956
882.219761	54189.578015	33.616973
882.839906	54255.988649	33.621991
883.818514	54328.942317	33.627008
884.566993	54407.970938	33.632026
885.655328	54477.375821	33.637044
885.997012	54559.013837	33.642061
886.943416	54625.339185	33.647079
887.920097	54707.426025	33.652096
888.679519	54805.654851	33.657114
889.481569	54879.973983	33.662132
890.322525	54973.001615	33.667149
891.407556	55061.047909	33.672167
891.965823	55147.335087	33.677184
892.810954	55236.528318	33.682202
893.843341	55316.863521	33.687220
894.478878	55416.740941	33.692237
895.438014	55504.550580	33.697255
896.931807	55588.377256	33.702272
897.906957	55688.928125	33.707290
898.938791	55766.468702	33.712308
899.577003	55854.940311	33.717325
900.361729	55939.594819	33.722343
901.622829	56030.947977	33.727360
902.274898	56115.703324	33.732378
903.547275	56181.370086	33.737396
904.623207	56285.847672	33.742413
905.222334	56372.569753	33.747431
906.579463	56444.231097	33.752448
907.290389	56535.380751	33.757466
908.012010	56619.578100	33.762484
908.950945	56704.874515	33.767501
909.741368	56785.305185	33.772519
910.917349	56865.245539	33.777536
911.499406	56963.703591	33.782554
912.910885	57057.285557	33.787572
913.479212	57137.115439	33.792589
914.388888	57226.128161	33.797607
915.491212	57313.570131	33.802624
916.556991	57396.611392	33.807642
917.312728	57480.362143	33.812660
918.351846	57567.455498	33.817677
919.127447	57656.876775	33.822695
920.144765	57749.287487	33.827712
920.633527	57827.677694	33.832730
922.041092	57920.567000	33.837748
922.980532	58008.963170	33.842765
923.784466	58094.950471	33.847783
924.968914	58177.060852	33.852800
925.685627	58260.843455	33.857818
926.517807	58347.828202	33.862836
927.368729	58440.328833	33.867853
928.266633	58522.063302	33.872871
929.404520	58610.677024	33.877888
930.028283	58691.085703	33.882906
930.989557	58793.344785	33.887924
931.604183	58848.773704	33.892941
931.934037	58955.948701	33.897959
933.651128	59036.235429	33.902976
934.348989	59119.687106	33.907994
935.071773	59193.123898	33.913012
936.122175	59304.037968	33.918029
936.542616	59386.796211	33.923047
937.882684	59454.620239	33.928064
938.555529	59567.998575	33.933082
939.468492	59653.552695	33.938100
940.775154	59735.050668	33.943117
941.546171	59843.969683	33.948135
942.779200	59925.480207	33.953152
943.723234	60030.587224	33.958170
944.542620	60116.802448	33.963188
945.750454	60211.872516	33.968205
946.640596	60308.657528	33.973223
947.544730	60399.050350	33.978240
948.205069	60503.718939	33.983258
949.595447	60570.724437	33.988276
950.648936	60689.486026	33.993293
951.645306	60786.910195	33.998311
952.360790	60858.618139	34.003328
953.251140	60976.125590	34.008346
954.178197	61072.555051	34.013364
955.427131	61135.707724	34.018381
956.094101	61273.558273	34.023399
957.312114	61335.497748	34.028416
958.122225	61451.937925	34.033434
958.773376	61527.460321	34.038452
960.191054	61638.986595	34.043469
960.851684	61722.976829	34.048487
962.024192	61826.188302	34.053504
963.115191	61924.661119	34.058522
964.111099	62019.859345	34.063540
965.149774	62113.781880	34.068557
965.814585	62207.511753	34.073575
966.918596	62306.053965	34.078592
968.048805	62417.330616	34.083610
969.103053	62507.441313	34.088628
970.322896	62597.017704	34.093645
970.753247	62691.466193	34.098663
971.943559	62799.912529	34.103680
972.722543	62889.055206	34.108698
973.961665	62979.075588	34.113716
974.972402	63092.023584	34.118733
976.172753	63187.788846	34.123751
977.033987	63260.884827	34.128768
977.718326	63367.678116	34.133786
978.617708	63465.008427	34.138804
979.901635	63561.851747	34.143821
980.334226	63661.597316	34.148839
981.588085	63760.855907	34.153856
982.593757	63849.509144	34.158874
983.550922	63941.366345	34.163892
984.252037	64027.116193	34.168909
984.889129	64109.355482	34.173927
986.374326	64215.249270	34.178944
986.986670	64310.949537	34.183962
987.802462	64387.025607	34.188980
989.023319	64480.899331	34.193997
989.637945	64594.749849	34.199015
990.779418	64689.284628	34.204032
991.642377	64792.612060	34.209050
992.736351	64893.768427	34.214068
993.649566	64991.281205	34.219085
994.645546	65099.705278	34.224103
995.996263	65193.053392	34.229120
996.365316	65304.051188	34.234138
997.358473	65419.870786	34.239156
998.630469	65535.090883	34.244173
999.714136	65635.924367	34.249191
1000.901329	65745.212298	34.254208
1001.817938	65849.395947	34.259226
1002.884335	65957.317831	34.264244
1003.606376	66058.413197	34.269261
1004.695364	66167.289630	34.274279
1006.194200	66268.303584	34.279296
1007.184945	66375.567134	34.284314
1007.782935	66479.612230	34.289332
1009.463416	66586.119768	34.294349
1010.118708	66699.587843	34.299367
1011.107880	66809.282865	34.304384
1011.723530	66911.893569	34.309402
1012.955712	67019.198100	34.314420
1013.994120	67126.499311	34.319437
1014.649665	67245.791604	34.324455
1015.978756	67346.336025	34.329472
1017.008371	67471.318671	34.334490
1017.893334	67591.562060	34.339508
1019.233741	67707.709745	34.344525
1020.310863	67808.871514	34.349543
1021.063752	67923.844210	34.354560
1022.307295	68037.520313	34.359578
1023.491873	68152.343570	34.364596
1024.586445	68251.799217	34.369613
1025.434269	68363.626043	34.374631
1026.595511	68484.241649	34.379648
1027.883193	68582.948095	34.384666
1029.104535	68704.458896	34.389684
1030.138995	68792.043779	34.394701
1031.043589	68911.072954	34.399719
1032.092669	69020.951026	34.404736
1032.930976	69121.367933	34.409754
1033.847223	69219.688149	34.414772
1035.143801	69318.605397	34.419789
1035.674847	69437.930962	34.424807
1036.908668	69545.590372	34.429824
1038.009905	69649.322877	34.434842
1038.631191	69765.205552	34.439860
1040.050644	69853.245704	34.444877
1040.891262	69955.182806	34.449895
1042.107790	70047.786008	34.454912
1042.986023	70143.962531	34.459930
1044.179700	70250.242270	34.464948
1045.064749	70361.411246	34.469965
1045.574879	70472.394085	34.474983
1047.159971	70569.963948	34.480000
1047.956975	70670.806054	34.485018
1048.763634	70776.771125	34.490036
1050.000594	70876.173275	34.495053
1050.861184	71013.361620	34.500071
1051.921461	71113.942986	34.505088
1053.006488	71223.315930	34.510106
1054.427257	71338.613174	34.515124
1055.743748	71429.905434	34.520141
1056.788643	71561.261750	34.525159
1057.821685	71648.884917	34.530176
1058.781343	71747.128764	34.535194
1059.763367	71878.756248	34.540212
1061.050135	71975.059981	34.545229
1062.023666	72080.708552	34.550247
1062.954883	72198.028476	34.555264
1064.266594	72308.426579	34.560282
1065.387690	72418.855617	34.565300
1066.705293	72531.471868	34.570317
1067.616064	72650.206785	34.575335
1068.618463	72752.309556	34.580352
1069.531430	72863.418686	34.585370
1070.377004	72979.145569	34.590388
1071.635652	73088.602319	34.595405
1072.887834	73204.790306	34.600423
1073.889224	73319.597107	34.605440
1074.754034	73439.550965	34.610458
1075.952639	73553.651619	34.615476
1077.130944	73646.069268	34.620493
1077.949223	73777.931281	34.625511
1079.235839	73884.013580	34.630528
1080.199152	74008.454389	34.635546
1080.904464	74145.493211	34.640564
1082.225394	74245.303349	34.645581
1083.277363	74372.468541	34.650599
1084.167478	74480.108413	34.655616
1085.309611	74615.109357	34.660634
1086.385374	74745.148426	34.665652
1087.486843	74870.198237	34.670669
1088.726407	74992.793877	34.675687
1089.919104	75114.822648	34.680704
1091.393554	75227.827312	34.685722
1092.195293	75343.549580	34.690740
1093.282978	75463.025110	34.695757
1094.011594	75586.482948	34.700775
1095.369335	75711.592031	34.705792
1096.551176	75817.454764	34.710810
1096.994701	75955.640881	34.715828
1098.760706	76049.227457	34.720845
1099.324873	76173.764127	34.725863
1100.200675	76280.436342	34.730880
1101.563874	76394.912496	34.735898
1102.463164	76528.365968	34.740916
1103.782295	76626.317525	34.745933
1104.578487	76757.981400	34.750951
1105.784284	76869.660237	34.755968
1106.959011	76995.716468	34.760986
1107.828586	77116.228717	34.766004
1109.167742	77235.782179	34.771021
1110.026848	77362.921070	34.776039
1111.114101	77492.558883	34.781056
1112.479803	77610.220580	34.786074
1113.655027	77746.735109	34.791092
1114.761371	77867.252077	34.796109
1116.020009	77996.562468	34.801127
1117.157836	78113.858814	34.806144
1118.860621	78225.883215	34.811162
1120.215921	78358.201705	34.816180
1121.361430	78465.771617	34.821197
1122.623410	78572.217476	34.826215
1123.371534	78682.449477	34.831232
1125.061655	78801.444350	34.836250
1125.929370	78919.420343	34.841268
1127.100000	79031.609646	34.846285
1128.307007	79147.352353	34.851303
1129.127872	79259.175036	34.856320
1130.338543	79370.013500	34.861338
1130.966700	79495.388321	34.866356
1132.319389	79614.580639	34.871373
1133.397878	79725.081750	34.876391
1134.602936	79869.803929	34.881408
1136.012894	79989.962745	34.886426
1137.001430	80111.466128	34.891444
1137.922610	80227.601710	34.896461
1139.020277	80351.725040	34.901479
1140.208417	80475.240541	34.906496
1141.886892	80601.118782	34.911514
1143.095819	80723.437760	34.916532
1144.032865	80837.216433	34.921549
1145.415927	80951.980460	34.926567
1146.252696	81068.292223	34.931584
1147.689359	81177.214394	34.936602
1148.649001	81307.446559	34.941620
1150.206487	81440.827367	34.946637
1151.086725	81555.548270	34.951655
1152.295683	81661.904753	34.956672
1153.407680	81791.685865	34.961690
1154.205161	81913.268137	34.966708
1155.685052	82019.823588	34.971725
1156.848248	82153.594077	34.976743
1157.696150	82279.096214	34.981760
1159.477693	82383.797558	34.986778
1160.364073	82496.727303	34.991796
1161.728991	82584.300733	34.996813
1162.849433	82688.451270	35.001831
1163.888688	82785.319827	35.006848
1165.106376	82895.316284	35.011866
1165.791438	83005.783653	35.016884
1167.119861	83109.833678	35.021901
1168.173619	83218.751565	35.026919
1169.167086	83331.953283	35.031936
1170.322366	83427.889675	35.036954
1171.112117	83586.062258	35.041972
1172.227538	83674.482835	35.046989
1173.485097	83815.601570	35.052007
1174.393103	83942.861684	35.057024
1175.642943	84059.889422	35.062042
1176.514730	84192.024918	35.067060
1177.870468	84306.748529	35.072077
1179.262376	84456.865808	35.077095
1180.320145	84572.839494	35.082112
1181.879568	84690.927929	35.087130
1183.056229	84850.388835	35.092148
1184.289176	84959.793042	35.097165
1185.406951	85094.860329	35.102183
1186.615562	85224.495584	35.107200
1187.928198	85355.898071	35.112218
1189.199050	85494.421005	35.117236
1190.605514	85601.682851	35.122253
1191.964949	85733.895868	35.127271
1192.621997	85866.663985	35.132288
1194.151044	85987.774127	35.137306
1195.114315	86127.905511	35.142324
1196.544245	86246.661822	35.147341
1197.636033	86378.036199	35.152359
1198.895165	86509.764155	35.157376
1200.517662	86627.157827	35.162394
1201.571330	86760.747349	35.167412
1202.679855	86888.454851	35.172429
1204.009596	87012.119092	35.177447
1205.091578	87123.860059	35.182464
1206.514188	87253.884660	35.187482
1207.610954	87394.534281	35.192500
1209.125082	87515.674446	35.197517
1210.050370	87633.228766	35.202535
1211.168107	87765.012232	35.207552
1212.382095	87891.216641	35.212570
1213.775018	88019.397861	35.217588
1214.917576	88143.281773	35.222605
1216.400352	88273.138579	35.227623
1217.365644	88402.452418	35.232640
1218.847492	88521.402808	35.237658
1219.982748	88651.481563	35.242676
1221.255479	88772.224544	35.247693
1222.527596	88900.714783	35.252711
1223.749674	89011.127970	35.257728
1225.093479	89145.343859	35.262746
1226.171037	89254.187685	35.267764
1227.489840	89367.629047	35.272781
1228.635143	89462.835372	35.277799
1229.585631	89585.069637	35.282816
1230.513481	89695.893560	35.287834
1231.453832	89821.153588	35.292852
1232.625159	89940.629132	35.297869
1234.179626	90060.436506	35.302887
1235.036351	90183.302474	35.307904
1236.334663	90308.780336	35.312922
1237.337007	90439.049057	35.317940
1238.374193	90552.996725	35.322957
1239.811520	90704.567165	35.327975
1241.070167	90844.492540	35.332992
1242.221072	90964.773805	35.338010
1243.462833	91117.345815	35.343028
1244.752974	91227.531773	35.348045
1246.381354	91381.422867	35.353063
1247.640302	91530.883433	35.358080
1248.739812	91640.760261	35.363098
1249.676765	91783.746905	35.368116
1250.865088	91937.066762	35.373133
1252.658881	92065.404201	35.378151
1254.030789	92203.258440	35.383168
1255.170190	92349.808965	35.388186
1256.616467	92477.615867	35.393204
1257.963440	92610.676178	35.398221
1259.000204	92744.691052	35.403239
1260.221113	92887.095790	35.408256
1261.857397	93023.762018	35.413274
1262.882417	93162.025268	35.418292
1264.366257	93302.898213	35.423309
1265.563862	93426.923563	35.428327
1266.905150	93569.984009	35.433344
1268.477292	93708.170017	35.438362
1269.957751	93843.759202	35.443380
1271.326562	93973.623751	35.448397
1272.432639	94105.396749	35.453415
1273.448143	94240.910470	35.458432
1274.755304	94365.347438	35.463450
1275.949856	94503.427640	35.468468
1277.171444	94640.119155	35.473485
1278.609839	94772.229117	35.478503
1279.666600	94917.013355	35.483520
1281.108376	95057.644772	35.488538
1282.174611	95194.908368	35.493556
1283.373795	95333.499005	35.498573
1285.107752	95464.819669	35.503591
1286.026642	95612.742494	35.508608
1287.590550	95746.470263	35.513626
1288.705834	95885.539422	35.518644
1290.118764	96028.003311	35.523661
1291.285850	96153.528892	35.528679
1292.866078	96298.485546	35.533696
1293.700974	96434.053907	35.538714
1295.148944	96547.005592	35.543732
1296.487147	96673.601245	35.548749
1297.696188	96806.746492	35.553767
1298.363507	96942.806341	35.558784
1300.098492	97051.868748	35.563802
1301.438231	97193.529263	35.568820
1302.098758	97322.602214	35.573837
1304.011576	97445.454388	35.578855
1305.080060	97598.167971	35.583872
1306.354480	97732.541873	35.588890
1307.788570	97861.184943	35.593908
1308.887524	98011.682289	35.598925
1310.363228	98126.162084	35.603943
1311.342350	98283.904905	35.608960
1312.827491	98416.281866	35.613978
1314.280465	98565.891523	35.618996
1315.383155	98708.345686	35.624013
1317.067262	98849.721387	35.629031
1318.368840	98990.747544	35.634048
1319.512728	99135.760069	35.639066
1321.103342	99275.426113	35.644084
1322.337987	99422.709936	35.649101
1324.038501	99558.538944	35.654119
1325.088031	99714.274885	35.659136
1326.446775	99850.438323	35.664154
1327.968000	99996.440232	35.669172
1328.896893	100136.520389	35.674189
1330.397749	100279.420852	35.679207
1331.732394	100426.834410	35.684224
1333.137740	100585.259248	35.689242
1334.144158	100734.707286	35.694260
1335.687939	100882.546060	35.699277
1337.004139	101022.747194	35.704295
1338.096111	101189.799193	35.709312
1339.672299	101323.861474	35.714330
1341.187363	101461.515446	35.719348
1342.319582	101627.014033	35.724365
1343.976593	101768.570164	35.729383
1345.171272	101922.342789	35.734400
1346.580058	102073.937421	35.739418
1348.251506	102221.536659	35.744436
1349.389945	102365.962912	35.749453
1351.213005	102503.460211	35.754471
1352.410380	102663.153503	35.759488
1354.089396	102793.221573	35.764506
1355.456412	102925.383773	35.769524
1356.302102	103090.425757	35.774541
1358.253851	103242.764282	35.779559
1359.617979	103379.991661	35.784576
1360.526255	103519.525995	35.789594
1362.227213	103654.246273	35.794612
1363.609513	103806.685296	35.799629
1365.132800	103949.028915	35.804647
1366.463707	104085.987274	35.809664
1367.575767	104219.304671	35.814682
1368.983578	104351.740524	35.819700
1370.051444	104477.827190	35.824717
1371.543965	104603.815399	35.829735
1372.962368	104729.550281	35.834752
1374.231571	104856.208138	35.839770
1375.619461	104999.149147	35.844788
1376.446238	105123.790458	35.849805
1377.969583	105251.441536	35.854823
1379.222698	105401.936988	35.859840
1380.348605	105541.670176	35.864858
1381.785491	105679.146172	35.869876
1382.655823	105834.983038	35.874893
1383.969848	105992.243918	35.879911
1385.472559	106157.487688	35.884928
1386.778295	106303.847993	35.889946
1388.002422	106466.853590	35.894964
1388.905375	106624.683923	35.899981
1390.841941	106782.249773	35.904999
1392.181851	106964.150324	35.910016
1393.772520	107122.488527	35.915034
1395.062944	107289.090230	35.920052
1396.447728	107453.804765	35.925069
1398.145457	107592.313558	35.930087
1399.795840	107784.651557	35.935104
1401.315011	107943.196401	35.940122
1402.383995	108104.528963	35.945140
1403.745487	108263.208561	35.950157
1405.389493	108419.540527	35.955175
1406.966281	108600.409479	35.960192
1407.949533	108765.494253	35.965210
1409.904206	108926.400408	35.970228
1411.207296	109090.164398	35.975245
1412.548553	109246.239680	35.980263
1414.119551	109419.317992	35.985280
1415.940814	109580.787681	35.990298
1417.644661	109726.523211	35.995316
1418.392773	109899.640764	36.000333
1419.853645	110052.815983	36.005351
1421.847205	110197.166437	36.010368
1422.996463	110380.718009	36.015386
1424.685717	110528.910196	36.020404
1425.905829	110690.546056	36.025421
1427.608103	110842.586503	36.030439
1428.974869	111001.751519	36.035456
1430.572426	111154.095376	36.040474
1432.218376	111300.602732	36.045492
1433.188351	111474.987436	36.050509
1434.781603	111625.891693	36.055527
1436.507573	111783.061409	36.060544
1438.016161	111928.632180	36.065562
1439.532409	112073.765823	36.070580
1440.932127	112232.718338	36.075597
1442.488644	112399.205086	36.080615
1443.708930	112531.145895	36.085632
1445.188154	112667.496363	36.090650
1446.666427	112809.646191	36.095668
1448.054878	112954.849617	36.100685
1449.310748	113075.045085	36.105703
1450.552183	113227.654554	36.110720
1451.614448	113370.133233	36.115738
1453.090617	113506.305210	36.120756
1454.428693	113663.573808	36.125773
1455.696213	113810.782860	36.130791
1457.098659	113972.075669	36.135808
1458.533351	114114.246198	36.140826
1459.896396	114273.388500	36.145844
1461.270753	114441.411858	36.150861
1462.838777	114603.239516	36.155879
1464.491122	114762.997346	36.160896
1465.788311	114927.934183	36.165914
1467.580968	115081.290365	36.170932
1469.190856	115243.571309	36.175949
1470.481091	115403.643975	36.180967
1471.666061	115566.614935	36.185984
1473.168658	115721.920370	36.191002
1474.583768	115893.428951	36.196020
1475.976363	116068.740881	36.201037
1477.786896	116240.429563	36.206055
1479.200916	116408.719295	36.211072
1480.766257	116561.341851	36.216090
1482.097626	116739.143614	36.221108
1483.748443	116915.230750	36.226125
1485.037947	117093.984993	36.231143
1486.459635	117257.593979	36.236160
1488.138335	117417.528982	36.241178
1489.383633	117600.801718	36.246196
1491.369270	117780.520166	36.251213
1492.995746	117954.054097	36.256231
1494.400670	118117.202711	36.261248
1496.076732	118284.393143	36.266266
1497.857803	118458.450437	36.271284
1499.015250	118633.196831	36.276301
1500.567837	118795.002970	36.281319
1502.119923	118961.932574	36.286336
1503.806003	119136.395774	36.291354
1505.832152	119297.192723	36.296372
1507.171917	119476.936988	36.301389
1508.902231	119630.925612	36.306407
1510.420458	119800.398765	36.311424
1511.802573	119969.926308	36.316442
1513.309191	120123.605137	36.321460
1514.938667	120274.460257	36.326477
1516.339604	120454.562495	36.331495
1517.949919	120606.024129	36.336512
1519.297853	120766.165405	36.341530
1520.977590	120939.451276	36.346548
1522.453218	121092.570841	36.351565
1523.392614	121251.260251	36.356583
1525.380916	121437.063656	36.361600
1526.568030	121577.174622	36.366618
1527.900580	121744.669870	36.371636
1529.381302	121892.056133	36.376653
1531.049311	122033.777565	36.381671
1532.328087	122196.116929	36.386688
1533.705555	122352.628330	36.391706
1535.512743	122499.092235	36.396724
1536.830583	122662.390814	36.401741
1538.164341	122818.937252	36.406759
1539.674483	122986.969447	36.411776
1541.192553	123154.165526	36.416794
1542.922837	123313.260982	36.421812
1544.228649	123482.519338	36.426829
1545.774684	123649.549440	36.431847
1547.447459	123827.123736	36.436864
1548.522210	124015.788210	36.441882
1550.324242	124182.160353	36.446900
1551.853633	124340.457905	36.451917
1553.235246	124535.005008	36.456935
1554.965681	124704.659640	36.461952
1556.405309	124882.594639	36.466970
1558.143947	125065.904533	36.471988
1560.055188	125239.232410	36.477005
1561.404595	125429.446508	36.482023
1563.367623	125602.439167	36.487040
1565.114480	125769.108582	36.492058
1566.694264	125939.301602	36.497076
1568.301111	126119.320895	36.502093
1569.857250	126310.534376	36.507111
1571.474729	126462.116918	36.512128
1572.906275	126647.639731	36.517146
1574.555977	126829.759677	36.522164
1576.222419	127003.897785	36.527181
1577.798724	127170.906925	36.532199
1579.498097	127367.704069	36.537216
1581.254229	127536.777017	36.542234
1582.721095	127704.275504	36.547252
1584.088343	127885.193268	36.552269
1585.432080	128064.583158	36.557287
1587.224330	128250.933646	36.562304
1588.698473	128436.018460	36.567322
1590.335348	128615.593408	36.572340
1591.950066	128795.312396	36.577357
1593.753905	128979.119684	36.582375
1595.347331	129146.556185	36.587392
1596.852507	129349.213113	36.592410
1598.497748	129531.149007	36.597428
1600.456027	129715.950139	36.602445
1601.496222	129890.168002	36.607463
1603.330836	130070.316414	36.612480
1604.937365	130257.127997	36.617498
1606.568515	130443.848241	36.622516
1608.436851	130625.071741	36.627533
1609.921352	130802.911406	36.632551
1611.599589	130969.825992	36.637568
1613.323678	131165.214639	36.642586
1614.608338	131317.484872	36.647604
1616.255126	131487.524177	36.652621
1617.893959	131631.846862	36.657639
1619.406490	131823.789607	36.662656
1620.822359	131960.180277	36.667674
1622.196133	132141.162718	36.672692
1623.927597	132307.633361	36.677709
1625.587015	132468.643082	36.682727
1627.354565	132644.346253	36.687744
1628.408868	132834.734234	36.692762
1630.197642	133000.034214	36.697780
1631.833384	133172.251995	36.702797
1633.033060	133355.651824	36.707815
1634.913101	133543.303346	36.712832
1636.348547	133733.358060	36.717850
1637.923787	133942.207435	36.722868
1640.127678	134120.904003	36.727885
1641.131968	134301.705470	36.732903
1643.274306	134483.873156	36.737920
1644.667290	134703.083628	36.742938
1646.326469	134865.500713	36.747956
1648.044016	135079.606840	36.752973
1649.920932	135257.462780	36.757991
1651.609989	135453.443984	36.763008
1653.067942	135664.871393	36.768026
1654.636991	135845.618196	36.773044
1656.531670	136061.186002	36.778061
1658.526786	136246.746119	36.783079
1660.345964	136444.753466	36.788096
1661.953076	136625.625795	36.793114
1663.745992	136829.405514	36.798132
1666.117173	136983.472125	36.803149
1667.095027	137212.106591	36.808167
1669.174179	137361.114808	36.813184
1670.744625	137572.297431	36.818202
1672.351105	137756.813729	36.823220
1674.357902	137935.603147	36.828237
1675.954487	138122.784473	36.833255
1678.107190	138321.778005	36.838272
1679.419577	138484.536466	36.843290
1680.845474	138685.523388	36.848308
1682.920328	138854.410348	36.853325
1683.992222	139051.147292	36.858343
1686.291183	139224.068696	36.863360
1687.740958	139447.905938	36.868378
1689.391306	139597.918673	36.873396
1691.277661	139821.334552	36.878413
1692.404634	139999.224290	36.883431
1694.913708	140158.494221	36.888448
1696.371292	140375.620424	36.893466
1698.137699	140560.179457	36.898484
1700.129368	140725.313596	36.903501
1701.226162	140950.295369	36.908519
1703.236981	141100.752664	36.913536
1704.816705	141307.233116	36.918554
1706.485181	141471.053920	36.923572
1708.024383	141626.125907	36.928589
1709.507491	141824.666126	36.933607
1710.966318	141963.276630	36.938624
1712.335405	142156.019811	36.943642
1714.334862	142323.962410	36.948660
1716.065859	142530.934145	36.953677
1717.823506	142689.500288	36.958695
1719.131225	142884.171628	36.963712
1720.861014	143085.634013	36.968730
1722.459769	143249.982455	36.973748
1724.280558	143469.937581	36.978765
1726.229276	143639.378396	36.983783
1727.952024	143824.990864	36.988800
1729.508014	144046.829993	36.993818
1731.127989	144215.793845	36.998836
1732.787039	144414.284922	37.003853
1734.370353	144628.937230	37.008871
1736.087938	144825.647154	37.013888
1737.944448	145041.412373	37.018906
1739.610745	145225.343747	37.023924
1741.471701	145452.442772	37.028941
1743.295410	145636.148776	37.033959
1745.221207	145864.343268	37.038976
1747.085925	146058.578582	37.043994
1748.644029	146255.259483	37.049012
1750.876275	146474.612872	37.054029
1752.569263	146683.507130	37.059047
1754.506065	146881.602223	37.064064
1756.154554	147086.031627	37.069082
1758.140738	147280.115776	37.074100
1759.978372	147489.005083	37.079117
1761.603206	147692.783009	37.084135
1763.259140	147878.011876	37.089152
1765.169623	148093.282457	37.094170
1766.778084	148308.323565	37.099188
1768.745392	148506.449336	37.104205
1770.578076	148713.154437	37.109223
1772.915310	148919.844154	37.114240
1774.715359	149111.560467	37.119258
1776.369293	149306.914031	37.124276
1778.347877	149499.973423	37.129293
1780.073294	149714.916676	37.134311
1781.830288	149906.872758	37.139328
1783.841350	150097.395157	37.144346
1785.629253	150295.344948	37.149364
1787.703302	150474.297918	37.154381
1789.100849	150674.885500	37.159399
1791.032286	150865.222223	37.164416
1792.908137	151067.840757	37.169434
1794.727825	151254.444945	37.174452
1796.465671	151444.080487	37.179469
1797.985922	151653.148673	37.184487
1799.894458	151838.055947	37.189504
1801.694012	152003.812551	37.194522
1803.385385	152196.984295	37.199540
1805.080162	152371.380426	37.204557
1806.640255	152540.106384	37.209575
1808.458060	152723.663813	37.214592
1810.485945	152887.486897	37.219610
1811.872052	153083.463482	37.224628
1813.736448	153256.125789	37.229645
1815.498279	153438.377520	37.234663
1817.408250	153631.446885	37.239680
1819.113333	153827.757586	37.244698
1820.547057	154002.634830	37.249716
1822.529340	154204.812014	37.254733
1823.853270	154415.754578	37.259751
1825.684439	154600.550105	37.264768
1827.494100	154806.181632	37.269786
1829.374230	155017.432735	37.274804
1831.341238	155224.347787	37.279821
1833.077082	155417.797440	37.284839
1835.256481	155648.759219	37.289856
1837.116886	155841.037707	37.294874
1838.816395	156057.383064	37.299892
1840.924475	156261.226323	37.304909
1843.069536	156479.240738	37.309927
1844.968743	156666.915047	37.314944
1846.714942	156879.111965	37.319962
1848.284553	157095.674735	37.324980
1850.354975	157277.974334	37.329997
1851.786306	157524.080595	37.335015
1853.938715	157715.727346	37.340032
1855.563263	157934.873424	37.345050
1857.477072	158129.895234	37.350068
1859.508271	158368.747986	37.355085
1861.571534	158579.560958	37.360103
1863.662210	158796.698412	37.365120
1865.545274	158998.133628	37.370138
1867.626613	159218.343890	37.375156
1869.408017	159419.911809	37.380173
1871.161017	159638.477626	37.385191
1872.932091	159838.388418	37.390208
1875.272882	160035.762506	37.395226
1876.862485	160266.062657	37.400244
1879.209952	160453.432731	37.405261
1880.977312	160680.258128	37.410279
1882.909721	160897.370331	37.415296
1885.275374	161088.405766	37.420314
1886.860443	161279.198369	37.425332
1888.889587	161498.302557	37.430349
1890.763213	161715.860271	37.435367
1892.652813	161890.007720	37.440384
1894.629679	162108.350383	37.445402
1896.323947	162306.524562	37.450420
1898.398646	162498.450743	37.455437
1900.581443	162721.038223	37.460455
1902.309086	162903.548299	37.465472
1904.162813	163099.393435	37.470490
1905.511431	163282.371410	37.475508
1907.726244	163456.639718	37.480525
1909.585741	163648.213039	37.485543
1911.062981	163838.262759	37.490560
1913.291502	164011.161878	37.495578
1914.667977	164203.639142	37.500596
1916.634703	164388.185989	37.505613
1918.299133	164588.546118	37.510631
1919.802348	164776.047421	37.515648
1922.121532	164979.527154	37.520666
1923.448076	165190.039593	37.525684
1925.527973	165390.921577	37.530701
1927.318654	165607.031951	37.535719
1928.964317	165819.894406	37.540736
1931.522490	166043.571398	37.545754
1933.250845	166257.957896	37.550772
1935.437396	166470.814351	37.555789
1937.342675	166681.243433	37.560807
1939.185112	166908.653947	37.565824
1941.317703	167117.692303	37.570842
1943.177414	167343.250947	37.575860
1944.845270	167555.739301	37.580877
1947.036980	167776.618373	37.585895
1949.007199	168006.970553	37.590912
1951.232621	168211.053628	37.595930
1953.366693	168458.543684	37.600948
1955.400566	168664.054824	37.605965
1957.737711	168868.034926	37.610983
1959.358342	169086.513533	37.616000
1961.771114	169300.288721	37.621018
1963.788099	169528.486418	37.626036
1966.137082	169729.057204	37.631053
1967.926161	169937.924649	37.636071
1969.667007	170159.015960	37.641088
1972.125394	170362.388632	37.646106
1973.898993	170588.005562	37.651124
1976.201433	170787.916976	37.656141
1978.074925	171007.064035	37.661159
1979.756635	171216.678463	37.666176
1981.979844	171419.967167	37.671194
1984.201173	171639.836372	37.676212
1986.103298	171840.641244	37.681229
1988.312635	172053.309628	37.686247
1989.837164	172269.474750	37.691264
1992.334590	172464.632292	37.696282
1994.191424	172672.095626	37.701300
1996.087535	172887.215732	37.706317
1998.299246	173099.661063	37.711335
2000.199806	173295.082333	37.716352
2002.370688	173491.806334	37.721370
2004.166848	173724.922174	37.726388
2006.154984	173916.450824	37.731405
2008.545742	174120.183559	37.736423
2010.337393	174344.728216	37.741440
2012.537208	174523.362841	37.746458
2014.342590	174724.705116	37.751476
2016.427949	174921.462411	37.756493
2018.137147	175080.894750	37.761511
2020.115952	175275.082738	37.766528
2022.023551	175463.447350	37.771546
2023.636271	175621.222563	37.776564
2025.928337	175855.007863	37.781581
2028.087250	176032.615387	37.786599
2029.648369	176209.011841	37.791616
2031.732418	176428.650121	37.796634
2033.564324	176608.874689	37.801652
2035.437570	176826.594835	37.806669
2037.840542	176995.249195	37.811687
2039.618486	177232.498567	37.816704
2041.448305	177455.227466	37.821722
2043.249521	177647.348903	37.826740
2045.271832	177867.613620	37.831757
2047.754723	178065.921519	37.836775
2049.542891	178293.495236	37.841792
2051.781455	178530.717009	37.846810
2053.965978	178716.197995	37.851828
2055.839779	178961.523702	37.856845
2058.434744	179152.625356	37.861863
2060.155661	179402.113926	37.866880
2062.813587	179607.392065	37.871898
2064.879321	179823.904717	37.876916
2067.066139	180041.693391	37.881933
2069.366641	180246.485772	37.886951
2070.984308	180482.878149	37.891968
2073.545229	180676.275858	37.896986
2075.493636	180888.612917	37.902004
2077.370132	181124.752086	37.907021
2080.213559	181315.684494	37.912039
2082.190818	181524.264508	37.917056
2084.657758	181749.071925	37.922074
2087.071843	181955.148627	37.927092
2088.957574	182155.790795	37.932109
2091.278560	182343.207203	37.937127
2093.307658	182551.872759	37.942144
2095.372303	182753.999203	37.947162
2097.660060	182954.619340	37.952180
2099.455222	183154.024321	37.957197
2101.444683	183360.746008	37.962215
2103.410968	183549.137424	37.967232
2106.034506	183770.555268	37.972250
2107.950530	183969.272272	37.977268
2109.971381	184160.982066	37.982285
2112.244929	184378.550353	37.987303
2114.332392	184577.674303	37.992320
2116.469982	184775.547683	37.997338
2118.658845	185004.653956	38.002356
2120.809001	185176.755895	38.007373
2122.910857	185378.545816	38.012391
2124.903267	185600.022110	38.017408
2127.217064	185780.031093	38.022426
2129.357839	185970.917511	38.027444
2131.022670	186119.625010	38.032461
2133.111541	186316.459687	38.037479
2135.067613	186482.493840	38.042496
2137.015925	186663.439872	38.047514
2139.309418	186859.609970	38.052532
2141.091117	187023.694198	38.057549
2143.326779	187230.445414	38.062567
2145.239109	187432.502933	38.067584
2147.442453	187614.287852	38.072602
2149.281430	187823.046170	38.077620
2151.253880	188024.373431	38.082637
2153.324492	188216.397042	38.087655
2155.406791	188449.877447	38.092672
2157.664932	188642.862886	38.097690
2159.834387	188859.517347	38.102708
2161.781998	189071.969519	38.107725
2163.885102	189297.786063	38.112743
2166.199081	189513.430792	38.117760
2168.844047	189716.156115	38.122778
2170.830066	189950.281077	38.127796
2172.564512	190171.693288	38.132813
2175.230625	190390.496824	38.137831
2177.541481	190627.365491	38.142848
2180.004731	190825.086253	38.147866
2182.010659	191059.188124	38.152884
2183.835108	191296.327602	38.157901
2186.804907	191502.232430	38.162919
2188.768299	191720.658555	38.167936
2191.275428	191935.001821	38.172954
2193.136620	192163.357679	38.177972
2195.540648	192385.283047	38.182989
2197.925161	192596.387106	38.188007
2200.162001	192822.160963	38.193024
2202.534803	193036.822273	38.198042
2204.950465	193254.460145	38.203060
2206.869598	193484.348600	38.208077
2209.485275	193697.857444	38.213095
2211.419485	193901.271457	38.218112
2213.864230	194123.033219	38.223130
2216.048790	194335.064825	38.228148
2218.490121	194552.171281	38.233165
2220.882012	194758.346409	38.238183
2223.098459	194983.879508	38.243200
2225.146225	195199.210894	38.248218
2227.678227	195403.716533	38.253236
2229.751682	195612.610914	38.258253
2231.909771	195822.203474	38.263271
2234.245897	196036.667723	38.268288
2236.750092	196248.085545	38.273306
2239.129332	196462.735125	38.278324
2240.854690	196671.333667	38.283341
2243.536100	196872.216973	38.288359
2245.789791	197088.615197	38.293376
2247.509893	197294.107520	38.298394
2249.833911	197478.778501	38.303412
2251.857039	197675.428578	38.308429
2253.905919	197854.280697	38.313447
2255.796072	198052.615975	38.318464
2257.863917	198245.796096	38.323482
2260.057121	198439.020513	38.328500
2262.090336	198639.937277	38.333517
2264.078424	198868.176322	38.338535
2266.167316	199072.639816	38.343552
2268.276017	199289.488983	38.348570
2270.782949	199504.613143	38.353588
2272.634719	199724.741461	38.358605
2274.839169	199972.307384	38.363623
2276.891179	200205.517599	38.368640
2279.286181	200429.180133	38.373658
2281.838967	200662.972954	38.378676
2284.055598	200909.766975	38.383693
2286.157795	201134.430826	38.388711
2288.265923	201375.075321	38.393728
2290.738343	201640.592553	38.398746
2293.418940	201869.813424	38.403764
2295.645339	202110.835882	38.408781
2298.120143	202361.746216	38.413799
2300.205707	202615.702356	38.418816
2302.834960	202853.249635	38.423834
2305.335604	203094.499442	38.428852
2307.681142	203342.832515	38.433869
2310.026893	203584.680199	38.438887
2312.155809	203828.695841	38.443904
2314.461033	204087.840923	38.448922
2316.818461	204335.237134	38.453940
2319.387672	204569.576937	38.458957
2321.842477	204818.470373	38.463975
2324.356902	205077.409063	38.468992
2326.513833	205311.741100	38.474010
2329.130287	205568.253952	38.479028
2331.331739	205817.496525	38.484045
2333.965065	206071.647816	38.489063
2336.050729	206319.501835	38.494080
2338.366713	206547.428425	38.499098
2340.759506	206804.223357	38.504116
2342.956095	207074.227304	38.509133
2345.470660	207316.140005	38.514151
2347.733797	207566.446538	38.519168
2350.052673	207819.601560	38.524186
2352.935052	208070.878376	38.529204
2354.866623	208317.127553	38.534221
2357.577225	208572.711798	38.539239
2360.119186	208805.333623	38.544256
2362.393997	209068.885193	38.549274
2364.766050	209321.644531	38.554292
2366.724010	209554.361792	38.559309
2369.223226	209828.341671	38.564327
2371.248109	210055.121656	38.569344
2373.734932	210331.809770	38.574362
2376.315568	210536.236236	38.579380
2378.245957	210782.952510	38.584397
2380.838266	210998.499614	38.589415
2383.042008	211209.487979	38.594432
2385.366344	211465.945225	38.599450
2387.730054	211667.794529	38.604468
2389.423126	211922.170085	38.609485
2392.001333	212156.931520	38.614503
2393.828710	212397.398855	38.619520
2396.067290	212661.288668	38.624538
2398.940527	212911.151882	38.629556
2400.845583	213160.623620	38.634573
2402.739855	213437.076381	38.639591
2405.714052	213691.916001	38.644608
2408.210391	213967.056770	38.649626
2410.483127	214244.417818	38.654644
2412.201961	214530.056687	38.659661
2415.000752	214773.565447	38.664679
2417.750703	215066.851186	38.669696
2419.904676	215354.836845	38.674714
2422.560299	215614.761975	38.679732
2425.268261	215922.036511	38.684749
2427.972868	216159.039376	38.689767
2430.349013	216469.809648	38.694784
2432.899900	216729.755629	38.699802
2435.562161	217026.174308	38.704820
2437.719841	217282.820151	38.709837
2440.486867	217581.535341	38.714855
2443.090108	217856.624134	38.719872
2445.183200	218156.451612	38.724890
2447.873062	218417.054762	38.729908
2450.572954	218689.985748	38.734925
2452.694189	218959.835312	38.739943
2455.485607	219265.117936	38.744960
2457.940838	219532.313871	38.749978
2460.845112	219795.249654	38.754996
2462.998679	220086.848036	38.760013
2465.484786	220369.849815	38.765031
2468.311715	220647.326251	38.770048
2470.365995	220940.492785	38.775066
2473.603152	221214.046420	38.780084
2475.775695	221479.097626	38.785101
2477.989995	221811.920836	38.790119
2480.732893	222096.754961	38.795136
2483.026613	222392.339777	38.800154
2485.863752	222656.807278	38.805172
2488.026633	222957.405069	38.810189
2490.656518	223224.167504	38.815207
2493.109502	223513.890559	38.820224
2495.386570	223798.246115	38.825242
2498.267815	224064.920800	38.830260
2500.961088	224347.003001	38.835277
2503.546803	224621.827487	38.840295
2505.884330	224897.212858	38.845312
2508.704495	225175.062240	38.850330
2510.863861	225411.711365	38.855348
2512.955155	225667.329833	38.860365
2515.716482	225907.288029	38.865383
2518.017062	226149.148443	38.870400
2519.932583	226406.727159	38.875418
2522.546891	226671.256022	38.880436
2524.705029	226931.959721	38.885453
2527.040285	227189.537838	38.890471
2529.389012	227462.961849	38.895488
2531.631241	227753.673104	38.900506
2534.245199	228022.841106	38.905524
2536.792473	228317.620161	38.910541
2539.459360	228600.978220	38.915559
2542.013688	228881.485225	38.920576
2544.359001	229186.711865	38.925594
2547.110017	229462.034034	38.930612
2549.845922	229757.219822	38.935629
2552.324935	230057.298120	38.940647
2555.049357	230343.217778	38.945664
2557.399470	230637.172358	38.950682
2560.135297	230935.308111	38.955700
2562.661955	231240.893997	38.960717
2565.118994	231535.952018	38.965735
2567.910854	231838.069220	38.970752
2570.275779	232150.515662	38.975770
2573.100575	232455.956728	38.980788
2576.041748	232755.564268	38.985805
2578.594238	233060.567877	38.990823
2581.386640	233365.432855	38.995840
2584.107854	233673.383231	39.000858
2586.894138	233962.732915	39.005876
2589.476078	234269.640529	39.010893
2592.127155	234569.883821	39.015911
2594.978251	234858.057556	39.020928
2597.284290	235166.230777	39.025946
2600.039633	235463.564828	39.030964
2602.645452	235757.799429	39.035981
2605.388556	236075.100420	39.040999
2607.857441	236365.955056	39.046016
2610.506727	236670.116248	39.051034
2613.325105	236975.394483	39.056052
2615.506328	237272.773908	39.061069
2618.153645	237584.532313	39.066087
2621.249503	237879.863610	39.071104
2623.409223	238200.666900	39.076122
2626.068771	238492.894110	39.081140
2628.875959	238806.281651	39.086157
2631.704374	239109.456207	39.091175
2634.421027	239420.954883	39.096192
2637.034320	239728.660884	39.101210
2639.742604	240039.273613	39.106228
2642.400230	240336.179451	39.111245
2644.959861	240643.007431	39.116263
2647.725630	240936.722725	39.121280
2650.045968	241247.806551	39.126298
2652.186420	241525.493532	39.131316
2654.967390	241795.789929	39.136333
2657.566126	242074.980377	39.141351
2659.901628	242357.743767	39.146368
2661.845338	242650.221894	39.151386
2664.602648	242931.700583	39.156404
2667.506260	243238.937901	39.161421
2669.944123	243532.406628	39.166439
2672.540851	243843.834270	39.171456
2674.726842	244139.300115	39.176474
2677.419538	244462.880820	39.181492
2680.401353	244774.503709	39.186509
2682.772652	245086.122441	39.191527
2685.419309	245412.252822	39.196544
2687.596781	245738.458313	39.201562
2690.471816	246050.431294	39.206580
2693.198449	246401.190064	39.211597
2695.728209	246755.460817	39.216615
2698.749109	247079.732407	39.221632
2701.347342	247424.138438	39.226650
2704.446238	247763.512790	39.231668
2706.986134	248107.142251	39.236685
2709.990335	248458.370108	39.241703
2713.052382	248795.161752	39.246720
2715.401708	249144.132625	39.251738
2718.432057	249479.787745	39.256756
2721.046759	249829.226157	39.261773
2723.741516	250183.047108	39.266791
2727.065325	250521.147304	39.271808
2729.509414	250865.661718	39.276826
2731.951559	251208.195839	39.281844
2735.099157	251574.267845	39.286861
2738.040935	251916.724278	39.291879
2741.014543	252265.425179	39.296896
2743.355954	252616.563871	39.301914
2746.262051	252959.002604	39.306932
2749.196644	253313.986005	39.311949
2751.804209	253677.709351	39.316967
2754.782772	254015.642451	39.321984
2757.394869	254368.926215	39.327002
2760.482980	254709.205590	39.332020
2763.426788	255068.229771	39.337037
2765.862137	255413.313139	39.342055
2769.178830	255756.352354	39.347072
2771.610702	256121.251191	39.352090
2774.434155	256457.993724	39.357108
2777.342986	256805.493856	39.362125
2779.809096	257156.265358	39.367143
2782.874019	257516.874927	39.372160
2785.237863	257862.100610	39.377178
2787.920284	258212.941116	39.382196
2791.083881	258573.130284	39.387213
2793.633039	258941.647729	39.392231
2797.016069	259280.922304	39.397248
2799.419229	259628.252733	39.402266
2802.324778	259952.209837	39.407284
2805.058083	260260.267134	39.412301
2807.252200	260590.688362	39.417319
2810.191008	260908.290690	39.422336
2813.037702	261233.630417	39.427354
2815.413759	261566.843709	39.432372
2818.136117	261886.285015	39.437389
2820.671545	262222.039503	39.442407
2823.581921	262570.055394	39.447424
2825.748791	262916.614426	39.452442
2828.776219	263268.804035	39.457460
2831.731197	263621.437345	39.462477
2834.241924	263987.528751	39.467495
2837.072230	264342.265588	39.472512
2840.103465	264718.487346	39.477530
2842.762786	265079.831363	39.482548
2845.796879	265456.307433	39.487565
2848.096035	265833.179662	39.492583
2851.278869	266197.134529	39.497600
2854.214056	266578.047427	39.502618
2856.693620	266969.524307	39.507636
2860.329326	267345.043061	39.512653
2863.248449	267729.973147	39.517671
2866.208707	268112.102650	39.522688
2868.822442	268502.695771	39.527706
2872.042666	268883.971742	39.532724
2874.895964	269282.097631	39.537741
2877.629549	269665.280170	39.542759
2880.406866	270056.737485	39.547776
2883.371145	270447.149276	39.552794
2886.162147	270850.595212	39.557812
2889.454974	271238.897695	39.562829
2892.266208	271636.294787	39.567847
2895.338635	272041.576538	39.572864
2898.626852	272422.208385	39.577882
2901.183042	272829.070935	39.582900
2904.655537	273226.668710	39.587917
2907.086256	273609.214869	39.592935
2910.267896	273995.986202	39.597952
2913.107181	274409.155139	39.602970
2915.909422	274802.210486	39.607988
2919.202287	275204.765282	39.613005
2922.111313	275585.787956	39.618023
2924.979860	275992.576109	39.623040
2927.819865	276386.387620	39.628058
2930.730308	276779.959322	39.633076
2934.290599	277181.557199	39.638093
2936.819841	277582.175083	39.643111
2940.058854	277977.650659	39.648128
2942.888157	278371.920834	39.653146
2945.862913	278774.347772	39.658164
2949.000782	279158.813979	39.663181
2951.973415	279561.545837	39.668199
2955.116896	279952.133093	39.673216
2957.945768	280325.038451	39.678234
2960.801888	280680.538050	39.683252
2963.425305	281040.062653	39.688269
2966.156555	281407.800689	39.693287
2968.968229	281774.585883	39.698304
2971.688176	282132.087791	39.703322
2974.242802	282503.536659	39.708340
2977.174244	282876.932507	39.713357
2979.731556	283257.627251	39.718375
2982.623924	283649.725541	39.723392
2985.471531	284029.611677	39.728410
2988.385631	284432.807109	39.733428
2991.551078	284828.417671	39.738445
2994.180008	285248.804645	39.743463
2997.578350	285646.765494	39.748480
3000.436030	286067.623497	39.753498
3003.304268	286471.332318	39.758516
3006.356841	286887.001757	39.763533
3009.167742	287303.902912	39.768551
3011.855843	287739.773616	39.773568
3014.952156	288162.750669	39.778586
3018.076980	288602.132930	39.783604
3021.580181	289030.048809	39.788621
3024.238928	289460.079161	39.793639
3027.449522	289902.621326	39.798656
3030.588702	290343.268904	39.803674
3033.226576	290780.794383	39.808692
3036.662557	291231.656247	39.813709
3039.686306	291677.197224	39.818727
3042.894084	292122.098633	39.823744
3046.500690	292560.356871	39.828762
3049.397170	292999.285553	39.833780
3052.665682	293445.241816	39.838797
3055.924693	293886.931115	39.843815
3059.076403	294321.574677	39.848832
3062.373298	294775.017484	39.853850
3064.940391	295216.203941	39.858868
3068.386172	295652.271583	39.863885
3071.381864	296107.029269	39.868903
3074.235748	296556.245310	39.873920
3077.848793	296999.878749	39.878938
3080.636662	297450.982902	39.883956
3083.987448	297883.148697	39.888973
3087.018754	298335.888695	39.893991
3090.249790	298785.598541	39.899008
3093.383198	299227.346561	39.904026
3096.546999	299673.914951	39.909044
3099.704436	300121.473834	39.914061
3102.939523	300567.418934	39.919079
3106.158200	301005.770396	39.924096
3109.117952	301452.442472	39.929114
3112.121540	301906.117097	39.934132
3115.312903	302337.331434	39.939149
3118.339923	302785.182891	39.944167
3121.574325	303222.865182	39.949184
3124.601098	303651.891902	39.954202
3127.713031	304080.472067	39.959220
3130.960569	304469.785228	39.964237
3133.820249	304886.591501	39.969255
3136.632098	305285.090210	39.974272
3139.822766	305692.595841	39.979290
3142.495703	306105.592478	39.984308
3145.923302	306514.734571	39.989325
3148.598463	306955.897304	39.994343
3151.625223	307370.256424	39.999360
3154.930604	307790.691571	40.004378
3157.381639	308230.107379	40.009396
3160.753634	308674.582934	40.014413
3163.920839	309116.676298	40.019431
3166.550941	309560.250027	40.024448
3169.769967	310016.200212	40.029466
3173.192072	310493.706201	40.034484
3176.164953	310936.052171	40.039501
3179.498464	311401.351276	40.044519
3182.453745	311866.200336	40.049536
3185.861575	312342.659520	40.054554
3188.756121	312825.776234	40.059572
3192.240811	313299.526824	40.064589
3195.675723	313778.616983	40.069607
3199.216335	314257.586678	40.074624
3202.115219	314728.959932	40.079642
3205.375329	315213.709736	40.084660
3208.860208	315686.611439	40.089677
3212.078404	316179.947965	40.094695
3215.360223	316664.179464	40.099712
3218.905259	317140.417375	40.104730
3222.097129	317623.236114	40.109748
3225.436782	318108.035500	40.114765
3228.816820	318591.987928	40.119783
3231.997270	319081.201354	40.124800
3235.166555	319564.877363	40.129818
3238.553018	320055.170582	40.134836
3241.839773	320527.952933	40.139853
3245.390043	321015.573782	40.144871
3248.392003	321512.421588	40.149888
3252.083773	321996.687713	40.154906
3255.219844	322481.902558	40.159924
3258.494869	322964.959418	40.164941
3261.910415	323450.403990	40.169959
3264.848297	323939.553004	40.174976
3268.363867	324422.385787	40.179994
3271.901941	324920.830668	40.185012
3275.193960	325395.109368	40.190029
3278.278086	325892.147222	40.195047
3281.240327	326386.382421	40.200064
3285.259598	326861.502544	40.205082
3288.044820	327349.385586	40.210100
3291.129442	327848.036491	40.215117
3294.405536	328335.911944	40.220135
3297.803518	328832.500783	40.225152
3301.246610	329309.195428	40.230170
3304.264533	329773.231793	40.235188
3307.518158	330220.366317	40.240205
3310.915299	330672.325717	40.245223
3313.548174	331130.853265	40.250240
3317.344595	331579.290399	40.255258
3320.299414	332046.014234	40.260276
3323.004990	332506.400746	40.265293
3326.155344	332977.683808	40.270311
3329.439581	333465.270270	40.275328
3332.469681	333929.455975	40.280346
3336.054589	334418.029375	40.285364
3339.468137	334903.401589	40.290381
3342.468510	335400.439996	40.295399
3345.699788	335912.419602	40.300416
3349.280740	336400.649384	40.305434
3352.454750	336915.550491	40.310452
3355.886465	337417.381008	40.315469
3359.178943	337925.044341	40.320487
3362.545231	338449.069338	40.325504
3366.340229	338964.008533	40.330522
3369.640523	339484.099981	40.335540
3373.217725	339999.750845	40.340557
3376.553604	340530.238214	40.345575
3379.784890	341061.118494	40.350592
3383.556510	341583.377811	40.355610
3386.522394	342111.675913	40.360628
3389.968851	342642.178519	40.365645
3393.841960	343178.778608	40.370663
3396.965903	343710.973149	40.375680
3400.604978	344238.917749	40.380698
3403.986158	344781.623778	40.385716
3407.507103	345317.422484	40.390733
3411.316496	345854.033865	40.395751
3414.252553	346397.760025	40.400768
3417.921724	346927.960491	40.405786
3421.347811	347473.046067	40.410804
3424.792337	348020.484490	40.415821
3428.133336	348565.395273	40.420839
3431.764307	349104.466748	40.425856
3435.619665	349642.888232	40.430874
3438.389194	350198.611747	40.435892
3442.411650	350729.761103	40.440909
3445.868010	351285.898028	40.445927
3449.163390	351830.428183	40.450944
3452.828473	352372.127367	40.455962
3456.455497	352904.434660	40.460980
3459.605592	353450.900409	40.465997
3463.276534	354001.771126	40.471015
3466.680431	354557.856561	40.476032
3470.542906	355091.500429	40.481050
3473.805879	355644.651881	40.486068
3477.474170	356179.431956	40.491085
3480.913689	356727.365518	40.496103
3483.996624	357277.253174	40.501120
3487.874168	357802.846102	40.506125
3490.853411	358302.971857	40.511130
3494.022678	358738.300394	40.516135
3497.175439	359135.126969	40.521140
3499.724651	359478.862723	40.526144
3502.191186	359763.980923	40.531149
3504.153543	360035.003650	40.536154
3506.114888	360229.483408	40.541159
3508.051625	360387.578576	40.546164
3509.231632	360512.840442	40.551168
3510.807281	360598.140380	40.556173
3511.901568	360651.072865	40.561178
3512.763547	360689.308906	40.566183
3513.651848	360706.573436	40.571188
3513.939542	360673.015891	40.576192
3514.982169	360636.031026	40.581197
3515.239890	360594.335502	40.586202
3515.717787	360522.731685	40.591207
3516.137752	360436.836314	40.596212
3516.036960	360340.412140	40.601216
3516.403797	360240.504083	40.606221
3516.656808	360130.969748	40.611226
3516.437389	360008.252405	40.616231
3516.586455	359870.972155	40.621236
3516.277880	359744.095054	40.626240
3516.562566	359602.950216	40.631245
3516.156539	359468.733801	40.636250
3515.893797	359334.163560	40.641255
3516.080435	359195.399564	40.646260
3515.554391	359050.233492	40.651264
3515.479173	358906.242612	40.656269
3515.413816	358781.334845	40.661274
3514.733911	358626.725633	40.666279
3514.902018	358495.876559	40.671284
3514.153721	358363.619737	40.676288
3514.231133	358230.315935	40.681293
3513.903922	358100.816466	40.686298
3513.475357	357971.154550	40.691303
3513.515608	357848.161711	40.696308
3512.994414	357735.359912	40.701312
3512.836136	357603.185914	40.706317
3512.779349	357489.241351	40.711322
3512.437164	357374.247401	40.716327
3512.242811	357254.522014	40.721332
3511.908236	357156.983393	40.726336
3511.983365	357045.409039	40.731341
3512.012855	356943.130076	40.736346
3511.370264	356834.086245	40.741351
3511.332806	356736.219911	40.746356
3510.830316	356634.787851	40.751360
3510.666917	356526.761860	40.756365
3510.477670	356452.229281	40.761370
3510.536601	356355.746608	40.766375
3510.332564	356260.781310	40.771380
3510.003412	356190.316705	40.776384
3509.883030	356105.949755	40.781389
3509.415706	356021.179443	40.786394
3509.332981	355945.280522	40.791399
3509.435543	355864.593369	40.796404
3509.039452	355805.463293	40.801408
3508.871307	355722.273878	40.806413
3508.808780	355656.092600	40.811418
3508.747261	355585.864780	40.816423
3508.779582	355530.331231	40.821428
3508.372092	355462.015669	40.826432
3508.378166	355400.887463	40.831437
3507.787993	355341.609391	40.836442
3507.803735	355292.923861	40.841447
3507.876125	355237.790837	40.846452
3507.586844	355181.900573	40.851456
3507.531982	355121.748714	40.856461
3507.298536	355071.982627	40.861466
3507.388637	355030.334375	40.866471
3507.554364	354977.425801	40.871476
3506.873560	354943.330373	40.876480
3507.260564	354901.660530	40.881485
3507.027319	354867.341606	40.886490
3506.913329	354821.806338	40.891495
3507.012368	354774.175998	40.896500
3506.831580	354738.499908	40.901504
3507.059978	354688.914928	40.906509
3506.711366	354653.621594	40.911514
3506.529604	354619.421611	40.916519
3506.549822	354580.965155	40.921524
3506.138242	354547.208638	40.926528
3506.581548	354510.950201	40.931533
3506.300600	354484.018758	40.936538
3506.193225	354447.363801	40.941543
3506.300189	354419.225797	40.946548
3505.946215	354405.921070	40.951552
3506.060588	354374.117213	40.956557
3506.059885	354342.789612	40.961562
3506.083040	354305.554041	40.966567
3506.330460	354272.507535	40.971572
3506.074132	354242.925372	40.976576
3506.275388	354213.041812	40.981581
3505.980603	354193.848931	40.986586
3505.621424	354170.161729	40.991591
3505.800315	354133.843032	40.996596
3505.621770	354109.261976	41.001600
3505.771172	354088.013802	41.006605
3505.880926	354068.247939	41.011610
3505.640050	354046.756056	41.016615
3505.715914	354020.378746	41.021620
3505.451338	353990.695946	41.026624
3505.645766	353974.937636	41.031629
3505.644952	353960.788038	41.036634
3505.736686	353936.825853	41.041639
3505.628158	353913.887835	41.046644
3505.593414	353878.697050	41.051648
3505.801816	353852.476847	41.056653
3505.828858	353828.881129	41.061658
3505.445347	353807.411696	41.066663
3505.775000	353787.738210	41.071668
3505.371244	353771.743562	41.076672
3505.178380	353749.327791	41.081677
3505.497224	353723.980791	41.086682
3505.114992	353710.654902	41.091687
3505.322028	353692.171434	41.096692
3505.155743	353683.035992	41.101696
3505.395461	353649.684917	41.106701
3505.282878	353641.711649	41.111706
3505.257155	353618.684064	41.116711
3505.655190	353596.200263	41.121716
3505.480019	353577.217289	41.126720
3505.157520	353550.877268	41.131725
3505.287513	353542.025806	41.136730
3504.943607	353528.592015	41.141735
3505.085173	353522.996248	41.146740
3504.910321	353501.010163	41.151744
3505.039378	353492.947774	41.156749
3504.743657	353487.777424	41.161754
3504.944685	353462.016281	41.166759
3505.154524	353447.476951	41.171764
3504.558021	353433.726774	41.176768
3504.802113	353420.836237	41.181773
3504.894773	353415.629932	41.186778
3504.570269	353396.110612	41.191783
3504.807918	353379.123714	41.196788
3504.844849	353364.484447	41.201792
3504.959006	353350.647353	41.206797
3505.077659	353353.937071	41.211802
3504.493724	353331.226650	41.216807
3505.077977	353325.840824	41.221812
3504.823561	353304.707069	41.226816
3504.773570	353297.029249	41.231821
3504.680248	353271.212746	41.236826
3504.829635	353270.145737	41.241831
3504.925339	353249.618299	41.246836
3504.668572	353242.125856	41.251840
3504.757850	353227.554625	41.256845
3504.805220	353219.148813	41.261850
3504.582397	353209.996777	41.266855
3504.939326	353195.612271	41.271860
3504.794023	353193.115770	41.276864
3505.141160	353172.777600	41.281869
3504.690808	353155.568550	41.286874
3504.910496	353145.633958	41.291879
3505.209875	353130.876788	41.296884
3504.729752	353131.054526	41.301888
3504.912659	353101.249580	41.306893
3504.938268	353101.245570	41.311898
3504.662630	353097.777133	41.316903
3504.818658	353065.227855	41.321908
3504.398955	353067.101168	41.326912
3504.770639	353054.928411	41.331917
3504.429420	353048.136433	41.336922
3504.491192	353027.359775	41.341927
3504.872682	353026.790512	41.346932
3504.447467	353019.375566	41.351936
3504.871693	352997.523611	41.356941
3504.701016	352998.823115	41.361946
3504.339143	352988.675035	41.366951
3504.810822	352969.894980	41.371956
3504.819337	352953.580410	41.376960
3504.778798	352953.001514	41.381965
3505.088438	352933.407222	41.386970
3504.836408	352911.178593	41.391975
3505.112655	352898.079247	41.396980
3504.570381	352884.065856	41.401984
3504.629202	352877.210614	41.406989
3504.978733	352864.583220	41.411994
3504.756298	352857.365242	41.416999
3504.688407	352837.118003	41.422004
3504.484956	352816.255942	41.427008
3504.563936	352824.845519	41.432013
3504.567616	352802.627320	41.437018
3504.862820	352797.974279	41.442023
3504.867975	352781.711088	41.447028
3504.593351	352781.118296	41.452032
3504.955095	352757.545533	41.457037
3505.170226	352742.547075	41.462042
3504.837378	352737.560669	41.467047
3504.973406	352721.454918	41.472052
3504.753527	352704.692832	41.477056
3504.567964	352705.867447	41.482061
3504.198870	352675.793228	41.487066
3504.494805	352678.851364	41.492071
3504.482109	352670.734909	41.497076
3504.473035	352673.510415	41.502080
3504.229857	352651.102129	41.507085
3504.392491	352646.342784	41.512090
3504.204575	352635.963536	41.517095
3504.478221	352628.692553	41.522100
3504.478538	352619.759637	41.527104
3504.192645	352620.492018	41.532109
3504.480840	352601.257291	41.537114
3504.495615	352591.838537	41.542119
3504.830659	352584.150644	41.547124
3504.480667	352586.242002	41.552128
3504.727018	352571.187660	41.557133
3504.692526	352556.406761	41.562138
3504.209545	352556.508602	41.567143
3504.604619	352535.984460	41.572148
3504.093482	352525.198190	41.577152
3503.986253	352522.975587	41.582157
3504.616813	352529.951018	41.587162
3504.183340	352506.071209	41.592167
3504.413420	352506.849272	41.597172
3504.497297	352506.759701	41.602176
3504.375775	352479.572973	41.607181
3504.435546	352482.617555	41.612186
3504.337340	352486.883258	41.617191
3504.645481	352451.917262	41.622196
3504.574284	352459.359941	41.627200
3504.453381	352446.984966	41.632205
3504.262352	352426.833387	41.637210
3504.332956	352434.253652	41.642215
3504.495450	352422.775519	41.647220
3504.426641	352408.330853	41.652224
3504.443410	352391.480356	41.657229
3504.488130	352386.459679	41.662234
3504.313266	352389.694058	41.667239
3504.540350	352378.002105	41.672244
3504.375739	352372.632769	41.677248
3504.403996	352349.087095	41.682253
3504.323579	352362.308395	41.687258
3504.344120	352343.523087	41.692263
3504.705404	352339.546710	41.697268
3504.224721	352339.317338	41.702272
3504.577399	352310.579459	41.707277
3504.381281	352310.737751	41.712282
3504.311973	352309.018145	41.717287
3504.237434	352288.135497	41.722292
3504.379167	352289.843731	41.727296
3504.224566	352290.097260	41.732301
3504.009519	352269.796718	41.737306
3504.429142	352270.035820	41.742311
3504.387564	352257.800961	41.747316
3504.402878	352262.684987	41.752320
3504.473299	352239.514349	41.757325
3504.443966	352239.595375	41.762330
3504.281619	352233.945716	41.767335
3504.323245	352208.412762	41.772340
3504.248157	352207.890219	41.777344
3504.470699	352214.421194	41.782349
3504.514519	352199.424215	41.787354
3504.464934	352185.460000	41.792359
3504.560474	352172.109092	41.797364
3504.434212	352160.294800	41.802368
3504.544728	352163.942180	41.807373
3504.504847	352149.136569	41.812378
3504.478004	352142.294775	41.817383
3504.528054	352128.569296	41.822388
3504.024700	352107.881617	41.827392
3504.731264	352103.647038	41.832397
3504.478332	352110.507693	41.837402
3504.673667	352077.620743	41.842407
3504.506806	352080.701176	41.847412
3504.321616	352065.562211	41.852416
3504.122720	352050.399959	41.857421
3504.338702	352042.298157	41.862426
3504.072388	352048.015679	41.867431
3504.335565	352023.847370	41.872436
3504.234456	352029.360626	41.877440
3504.380014	352015.823620	41.882445
3504.312814	352007.130327	41.887450
3504.127104	351995.299946	41.892455
3504.482917	351985.750821	41.897460
3504.173591	351983.560144	41.902464
3504.257672	351972.450613	41.907469
3504.158271	351960.886532	41.912474
3504.089318	351971.230245	41.917479
3504.627349	351969.720018	41.922484
3504.333475	351959.866392	41.927488
3504.333679	351952.994847	41.932493
3504.445487	351942.084528	41.937498
3504.435803	351936.334353	41.942503
3504.599777	351932.694541	41.947508
3504.218492	351917.942838	41.952512
3504.257388	351897.805610	41.957517
3504.420308	351902.691784	41.962522
3504.412292	351896.305086	41.967527
3504.451979	351877.491137	41.972532
3504.192671	351880.153542	41.977536
3504.174644	351865.624350	41.982541
3504.439049	351859.754486	41.987546
3504.263151	351853.216170	41.992551
3504.316772	351847.939533	41.997556
3504.210898	351831.693603	42.002560
3504.286946	351835.906360	42.007565
3504.102815	351821.683367	42.012570
3504.186818	351825.182261	42.017575
3504.613696	351801.827831	42.022580
3504.064313	351799.853248	42.027584
3504.282669	351802.643746	42.032589
3504.224512	351784.659641	42.037594
3504.049085	351782.447788	42.042599
3504.425224	351770.452186	42.047604
3504.186520	351784.105856	42.052608
3503.846037	351756.673422	42.057613
3504.023782	351742.876756	42.062618
3504.041949	351751.628821	42.067623
3503.996041	351747.844024	42.072628
3504.005121	351744.534090	42.077632
3504.135294	351746.116918	42.082637
3504.103041	351729.833868	42.087642
3503.662000	351731.914203	42.092647
3504.441859	351731.281949	42.097652
3504.478728	351726.186100	42.102656
3504.179200	351711.039660	42.107661
3504.058387	351710.498891	42.112666
3504.065393	351714.111765	42.117671
3504.467330	351699.567037	42.122676
3504.225487	351699.707109	42.127680
3504.106655	351683.564984	42.132685
3504.251563	351677.943044	42.137690
3504.089784	351677.103347	42.142695
3504.179854	351658.179554	42.147700
3504.089444	351663.233050	42.152704
3504.105450	351661.398135	42.157709
3504.047246	351676.244914	42.162714
3504.108009	351646.916568	42.167719
3504.183745	351650.340429	42.172724
3504.028724	351646.191119	42.177728
3504.177626	351637.667205	42.182733
3504.306751	351621.307710	42.187738
3504.080320	351622.666962	42.192743
3504.344989	351611.986914	42.197748
3504.100664	351615.257771	42.202752
3504.269740	351604.516483	42.207757
3504.138043	351594.637151	42.212762
3504.093215	351593.626262	42.217767
3503.995756	351582.901654	42.222772
3504.008889	351580.380030	42.227776
3504.125141	351566.516689	42.232781
3504.241180	351567.465498	42.237786
3503.952670	351558.934369	42.242791
3504.021144	351558.872682	42.247796
3503.819306	351558.879178	42.252800
3504.202680	351541.588702	42.257805
3504.131370	351546.053831	42.262810
3503.900844	351550.467778	42.267815
3504.358914	351539.069980	42.272820
3504.235266	351532.116160	42.277824
3504.211267	351527.895227	42.282829
3504.614966	351528.951263	42.287834
3504.262979	351515.798191	42.292839
3504.430453	351492.993644	42.297844
3504.326749	351496.140476	42.302848
3504.432336	351477.646825	42.307853
3504.242434	351470.907073	42.312858
3504.044566	351471.829156	42.317863
3504.357921	351463.610072	42.322868
3503.991545	351455.880201	42.327872
3504.018954	351442.438079	42.332877
3504.189717	351453.711113	42.337882
3504.097789	351436.495742	42.342887
3504.438067	351416.463392	42.347892
3504.334838	351423.300468	42.352896
3504.537358	351416.066015	42.357901
3504.492788	351390.724451	42.362906
3503.973321	351387.523501	42.367911
3503.966812	351371.923436	42.372916
3503.874361	351373.770523	42.377920
3503.904901	351375.114608	42.382925
3504.038541	351352.544404	42.387930
3504.068612	351367.199160	42.392935
3504.153924	351361.153950	42.397940
3504.272479	351366.479845	42.402944
3504.376524	351344.652379	42.407949
3504.257848	351332.684002	42.412954
3504.003137	351342.242787	42.417959
3504.160279	351327.533055	42.422964
3504.012535	351301.647848	42.427968
3503.769148	351304.129611	42.432973
3504.017754	351305.184719	42.437978
3504.187616	351303.961731	42.442983
3504.663732	351295.462386	42.447988
3504.510285	351276.958714	42.452992
3504.208737	351265.502792	42.457997
3504.268693	351265.747857	42.463002
3504.040580	351249.495625	42.468007
3504.017396	351237.741185	42.473012
3504.001140	351242.579394	42.478016
3504.136589	351246.248345	42.483021
3504.151253	351225.656587	42.488026
3504.110673	351228.920709	42.493031
3504.114989	351224.008112	42.498036
3504.183055	351225.193565	42.503040
3504.267245	351207.619422	42.508045
3504.255490	351198.077364	42.513050
3503.865282	351189.918562	42.518055
3504.279395	351187.791640	42.523060
3504.368371	351191.315239	42.528064
3503.991157	351167.247782	42.533069
3504.107321	351159.187079	42.538074
3503.944216	351170.436600	42.543079
3504.178099	351161.670121	42.548084
3503.767205	351155.245223	42.553088
3504.240668	351137.533166	42.558093
3504.123175	351143.303609	42.563098
3503.763908	351152.522648	42.568103
3504.250952	351138.804184	42.573108
3503.973104	351135.539572	42.578112
3504.041509	351130.540483	42.583117
3504.226828	351126.057373	42.588122
3504.053184	351131.225880	42.593127
3504.263937	351126.636947	42.598132
3503.657379	351105.456184	42.603136
3503.726696	351098.446351	42.608141
3503.738464	351091.063857	42.613146
3503.748229	351099.944609	42.618151
3504.090536	351085.027384	42.623156
3503.917968	351103.684540	42.628160
3503.974366	351106.169820	42.633165
3504.367818	351104.478821	42.638170
3504.235587	351079.659980	42.643175
3504.002822	351080.536686	42.648180
3504.131651	351089.195013	42.653184
3503.904038	351067.776175	42.658189
3504.060024	351044.107933	42.663194
3503.893480	351057.419522	42.668199
3504.023887	351051.087192	42.673204
3504.203595	351060.144690	42.678208
3503.957208	351050.792402	42.683213
3504.158995	351033.326865	42.688218
3504.157734	351026.786292	42.693223
3504.245002	351008.957092	42.698228
3504.250564	351027.357058	42.703232
3504.025350	351010.493480	42.708237
3504.200831	350996.976938	42.713242
3504.184116	350995.579834	42.718247
3504.075237	350991.448630	42.723252
3504.135221	350989.759443	42.728256
3504.221398	350976.104310	42.733261
3504.070225	350971.165369	42.738266
3503.908308	350973.685169	42.743271
3504.228664	350963.047090	42.748276
3504.150775	350953.540895	42.753280
3503.931437	350933.444130	42.758285
3504.051532	350932.025395	42.763290
3503.852544	350936.536210	42.768295
3504.126793	350935.907527	42.773300
3504.037991	350931.594990	42.778304
3503.979331	350914.374193	42.783309
3504.215353	350921.895771	42.788314
3503.835101	350925.111806	42.793319
3504.117490	350913.410792	42.798324
3504.022143	350900.115195	42.803329
3504.208457	350893.494051	42.808333
3504.224850	350891.073682	42.813338
3504.041772	350894.156746	42.818343
3504.181141	350862.906746	42.823348
3503.788409	350859.202165	42.828353
3504.131674	350847.873274	42.833357
3504.405680	350856.432335	42.838362
3503.924254	350853.556199	42.843367
3504.088896	350823.701969	42.848372
3503.715382	350826.789691	42.853377
3504.026745	350822.846546	42.858381
3504.318401	350826.083621	42.863386
3504.213328	350835.084374	42.868391
3504.221294	350816.453224	42.873396
3504.167904	350801.954787	42.878401
3504.291029	350805.396660	42.883405
3504.211766	350792.302100	42.888410
3504.092331	350784.634896	42.893415
3504.344922	350773.982043	42.898420
3503.853496	350781.847697	42.903425
3503.848916	350784.113576	42.908429
3504.289964	350763.225179	42.913434
3504.228075	350759.086528	42.918439
3504.246676	350744.500342	42.923444
3503.962953	350749.508132	42.928449
3504.102003	350728.820168	42.933453
3503.868508	350721.985412	42.938458
3503.610672	350723.680511	42.943463
3503.797288	350716.601183	42.948468
3503.844385	350709.238502	42.953473
3503.832921	350716.264767	42.958477
3503.964916	350713.826115	42.963482
3503.635823	350728.359668	42.968487
3503.909372	350709.890102	42.973492
3503.522052	350708.068013	42.978497
3503.783212	350709.630164	42.983501
3503.722369	350710.836008	42.988506
3503.742176	350702.612313	42.993511
3503.873567	350706.129239	42.998516
3503.965752	350712.350144	43.003521
3503.910210	350724.422630	43.008525
3503.993253	350709.215428	43.013530
3503.988522	350704.151509	43.018535
3504.013760	350699.668220	43.023540
3504.114643	350688.301261	43.028545
3504.052573	350688.845578	43.033549
3504.049384	350687.115467	43.038554
3503.690201	350676.050292	43.043559
3503.790259	350665.930547	43.048564
3503.694309	350658.590473	43.053569
3503.842942	350660.552177	43.058573
3503.781678	350659.874728	43.063578
3503.816960	350660.963573	43.068583
3503.575322	350670.876721	43.073588
3503.597242	350667.641043	43.078593
3503.687251	350665.819846	43.083597
3504.222489	350673.574115	43.088602
3503.737841	350659.830987	43.093607
3503.918210	350638.907400	43.098612
3503.777812	350644.732418	43.103617
3503.704902	350644.693081	43.108621
3503.939340	350650.204333	43.113626
3503.916378	350637.482597	43.118631
3504.199201	350648.432674	43.123636
3503.700941	350650.903857	43.128641
3503.559588	350627.307890	43.133645
3503.551101	350619.114106	43.138650
3503.511026	350631.693184	43.143655
3503.976507	350628.590988	43.148660
3504.020946	350630.925476	43.153665
3503.973174	350629.965936	43.158669
3504.065610	350623.206895	43.163674
3504.269651	350632.566028	43.168679
3504.163828	350613.723739	43.173684
3504.241685	350610.784625	43.178689
3504.394891	350600.147449	43.183693
3504.340125	350590.255772	43.188698
3504.139279	350586.240879	43.193703
3504.244702	350572.404446	43.198708
3504.089043	350566.702653	43.203713
3504.208537	350555.485428	43.208717
3504.238698	350543.544249	43.213722
3503.804350	350544.936397	43.218727
3503.927847	350537.103499	43.223732
3504.068461	350534.205361	43.228737
3504.147069	350525.717835	43.233741
3504.054911	350510.741882	43.238746
3504.106226	350514.627791	43.243751
3504.144892	350496.729754	43.248756
3504.086658	350513.511123	43.253761
3503.927840	350492.437494	43.258765
3504.262640	350475.663375	43.263770
3503.855380	350473.182707	43.268775
3503.957473	350475.100874	43.273780
3503.550892	350488.603254	43.278785
3503.698915	350489.597927	43.283789
3503.927429	350485.184288	43.288794
3503.857478	350464.911028	43.293799
3503.711544	350457.706083	43.298804
3503.739513	350457.905307	43.303809
3503.552290	350459.080234	43.308813
3503.636972	350457.768889	43.313818
3503.670011	350463.515606	43.318823
3503.715529	350461.065163	43.323828
3503.652497	350463.696608	43.328833
3503.783826	350479.277280	43.333837
3503.902366	350471.394254	43.338842
3503.608047	350471.669879	43.343847
3503.568264	350469.945546	43.348852
3503.902288	350475.135662	43.353857
3503.961973	350463.189798	43.358861
3503.914850	350444.236367	43.363866
3503.666054	350444.835657	43.368871
3504.047546	350440.474184	43.373876
3503.914054	350448.436007	43.378881
3503.804856	350447.308018	43.383885
3504.105482	350436.952915	43.388890
3503.646411	350431.706288	43.393895
3503.758723	350427.590975	43.398900
3504.121115	350416.258969	43.403905
3503.963600	350419.668880	43.408909
3503.863690	350425.258463	43.413914
3503.782496	350427.689173	43.418919
3503.806441	350425.165786	43.423924
3504.097219	350430.362744	43.428929
3503.565526	350399.702131	43.433933
3504.125217	350391.825706	43.438938
3503.780699	350399.490035	43.443943
3503.849357	350396.628716	43.448948
3503.716319	350403.903299	43.453953
3504.081971	350402.751142	43.458957
3504.087156	350392.111875	43.463962
3503.726723	350389.242037	43.468967
3504.090428	350367.729442	43.473972
3503.994109	350371.027878	43.478977
3503.862331	350378.913087	43.483981
3504.232691	350367.478009	43.488986
3504.094140	350350.346016	43.493991
3503.981185	350330.970288	43.498996
3504.382579	350335.513493	43.504001
3504.059491	350339.687662	43.509005
3504.157615	350340.690226	43.514010
3504.172654	350331.500093	43.519015
3504.014001	350325.926002	43.524020
3503.754905	350324.490845	43.529025
3503.901421	350324.620427	43.534029
3503.803967	350313.259293	43.539034
3503.675320	350297.500069	43.544039
3503.817450	350291.674817	43.549044
3503.767725	350286.745228	43.554049
3504.104831	350288.524444	43.559053
3503.850448	350281.209365	43.564058
3504.064502	350293.035718	43.569063
3504.002923	350282.127024	43.574068
3504.040605	350259.418829	43.579073
3503.709936	350263.110633	43.584077
3503.913635	350253.457995	43.589082
3503.984305	350258.257099	43.594087
3503.938092	350263.125581	43.599092
3504.023013	350260.821606	43.604097
3503.939831	350246.734946	43.609101
3503.981438	350236.980675	43.614106
3503.722914	350234.680091	43.619111
3504.176429	350235.219258	43.624116
3504.027559	350241.910992	43.629121
3504.072486	350248.546638	43.634125
3503.820520	350217.409034	43.639130
3503.638656	350215.503546	43.644135
3503.708078	350205.184951	43.649140
3504.010578	350208.369446	43.654145
3503.984803	350211.249523	43.659149
3503.885493	350211.519771	43.664154
3503.750078	350223.655897	43.669159
3503.902826	350209.302870	43.674164
3503.856691	350197.042813	43.679169
3504.046945	350193.271475	43.684173
3504.023417	350183.298433	43.689178
3503.715295	350188.106523	43.694183
3503.991752	350185.390499	43.699188
3504.148253	350194.960831	43.704193
3503.939847	350189.801808	43.709197
3504.128721	350167.960459	43.714202
3503.518195	350166.657208	43.719207
3503.854519	350155.761937	43.724212
3504.091347	350159.542191	43.729217
3504.017012	350166.069445	43.734221
3504.188057	350146.674206	43.739226
3503.941377	350141.546680	43.744231
3503.979426	350131.512991	43.749236
3504.045450	350129.491959	43.754241
3504.080925	350134.067578	43.759245
3504.418402	350130.247511	43.764250
3503.865197	350123.361416	43.769255
3504.180010	350100.329383	43.774260
3504.210458	350103.073322	43.779265
3503.803555	350096.902177	43.784269
3504.039620	350064.669292	43.789274
3503.804556	350076.592143	43.794279
3504.084927	350070.465052	43.799284
3503.792998	350076.568596	43.804289
3504.296925	350072.544053	43.809293
3504.131341	350051.013204	43.814298
3503.539616	350051.463102	43.819303
3503.769743	350047.125527	43.824308
3503.959097	350038.416810	43.829313
3503.541371	350036.675858	43.834317
3504.043088	350032.218993	43.839322
3503.858940	350038.814525	43.844327
3503.695366	350045.737667	43.849332
3503.769653	350054.506586	43.854337
3503.859583	350023.823844	43.859341
3504.107759	350016.709243	43.864346
3503.809676	350017.647194	43.869351
3503.769759	350018.646135	43.874356
3503.473752	350020.220035	43.879361
3503.771235	350009.585386	43.884365
3504.120816	350011.362640	43.889370
3503.940876	350015.361496	43.894375
3504.189018	350000.738823	43.899380
3504.080110	349996.022173	43.904385
3503.880189	349993.126938	43.909389
3504.207029	349980.222495	43.914394
3503.835323	349989.392794	43.919399
3503.786786	349978.252917	43.924404
3504.137810	349957.683858	43.929409
3503.786093	349959.877393	43.934413
3504.223797	349949.093310	43.939418
3503.936199	349969.423362	43.944423
3503.795339	349962.090294	43.949428
3503.868557	349948.538757	43.954433
3503.855748	349932.404800	43.959437
3504.002347	349919.808799	43.964442
3503.729269	349925.069492	43.969447
3503.660996	349925.563895	43.974452
3503.776525	349927.912626	43.979457
3504.011143	349926.221250	43.984461
3504.326882	349929.505473	43.989466
3504.109868	349910.298753	43.994471
3504.288234	349893.040163	43.999476
3504.040849	349896.540667	44.004481
3503.702389	349901.328127	44.009485
3504.060420	349890.302116	44.014490
3503.929204	349880.956871	44.019495
3503.581985	349876.965065	44.024500
3503.844283	349879.952326	44.029505
3503.921400	349878.133141	44.034509
3503.854404	349881.732384	44.039514
3503.868718	349891.910624	44.044519
3504.060848	349875.846057	44.049524
3503.826966	349859.517967	44.054529
3504.037923	349851.467536	44.059533
3504.093038	349846.444979	44.064538
3503.908462	349847.390439	44.069543
3503.804316	349836.717445	44.074548
3504.060705	349845.508512	44.079553
3503.949923	349834.811116	44.084557
3503.734880	349819.548986	44.089562
3503.693960	349823.958549	44.094567
3503.955215	349818.445280	44.099572
3503.692076	349825.027874	44.104577
3503.463640	349825.649402	44.109581
3503.477882	349821.447743	44.114586
3503.203860	349828.770141	44.119591
3503.397107	349824.871048	44.124596
3503.588003	349827.055162	44.129601
3503.498896	349823.836986	44.134605
3503.650095	349835.138900	44.139610
3503.646969	349838.982561	44.144615
3503.884761	349822.401736	44.149620
3503.793747	349833.411076	44.154625
3503.504566	349841.652111	44.159629
3503.790666	349829.364901	44.164634
3503.535462	349843.454337	44.169639
3503.861789	349845.184370	44.174644
3503.518186	349822.485368	44.179649
3503.746969	349817.664415	44.184653
3503.870919	349814.183496	44.189658
3503.741586	349817.105416	44.194663
3503.963182	349812.463757	44.199668
3503.709073	349811.664077	44.204673
3503.427536	349818.402287	44.209677
3503.975620	349809.840432	44.214682
3503.906074	349814.152717	44.219687
3503.668389	349819.967751	44.224692
3503.845499	349824.139237	44.229697
3503.914227	349810.461120	44.234701
3504.215303	349807.613930	44.239706
3503.898133	349807.231439	44.244711
3504.133607	349791.643568	44.249716
3504.226807	349795.064785	44.254721
3503.778058	349788.671159	44.259725
3503.857937	349766.286955	44.264730
3503.912565	349759.482882	44.269735
3503.938933	349750.138154	44.274740
3503.595522	349766.837579	44.279745
3503.633693	349763.548376	44.284749
3503.810645	349771.741183	44.289754
3503.817423	349776.957648	44.294759
3503.995427	349758.986439	44.299764
3503.771584	349741.307813	44.304769
3503.728702	349737.980519	44.309773
3504.276895	349720.434349	44.314778
3503.804818	349735.525245	44.319783
3503.807038	349728.118624	44.324788
3503.803299	349734.151195	44.329793
3503.965827	349740.259286	44.334797
3504.232810	349708.428524	44.339802
3503.836338	349702.204783	44.344807
3503.946671	349692.897673	44.349812
3503.961414	349711.245729	44.354817
3503.712324	349708.510960	44.359821
3503.858998	349702.099549	44.364826
3503.951665	349695.620321	44.369831
3503.805810	349681.365264	44.374836
3503.800499	349670.880224	44.379841
3503.854317	349676.012909	44.384845
3504.127153	349675.002667	44.389850
3503.827332	349679.834940	44.394855
3504.188686	349666.924967	44.399860
3504.197827	349646.511644	44.404865
3503.915735	349641.491474	44.409869
3504.022393	349634.602807	44.414874
3503.729830	349641.037366	44.419879
3503.810711	349651.154224	44.424884
3503.882066	349653.026376	44.429889
3503.899033	349639.025533	44.434893
3504.206705	349616.732513	44.439898
3503.379843	349613.732760	44.444903
3503.354666	349622.008446	44.449908
3503.654748	349608.064643	44.454913
3503.625542	349614.253961	44.459917
3503.738912	349616.094021	44.464922
3503.550577	349627.144238	44.469927
3503.750008	349621.437113	44.474932
3503.944931	349618.148572	44.479937
3503.623870	349625.554787	44.484941
3503.998194	349625.750162	44.489946
3503.681895	349627.200024	44.494951
3503.617191	349610.946921	44.499956
3503.776819	349602.548249	44.504961
3503.708990	349591.029574	44.509965
3503.720258	349588.813568	44.514970
3503.586056	349585.882472	44.519975
3503.963254	349594.323613	44.524980
3504.248860	349596.645471	44.529985
3503.396791	349597.187432	44.534989
3503.849644	349589.276880	44.539994
3503.847980	349590.906065	44.544999
3504.129557	349591.141553	44.550004
3503.955298	349565.743288	44.555009
3503.795105	349566.913960	44.560013
3503.996997	349563.777022	44.565018
3503.728163	349573.949180	44.570023
3503.883750	349565.372983	44.575028
3503.819051	349568.641017	44.580033
3503.569371	349585.071166	44.585037
3504.005947	349565.913709	44.590042
3503.855862	349549.877695	44.595047
3503.529596	349539.341564	44.600052
3503.696948	349534.988421	44.605057
3503.804573	349548.053424	44.610061
3503.707254	349541.527858	44.615066
3503.861195	349548.044549	44.620071
3504.003846	349541.430145	44.625076
3503.928764	349550.350014	44.630081
3503.521363	349531.707737	44.635085
3503.734699	349505.560984	44.640090
3504.121873	349514.636844	44.645095
3503.731673	349510.880868	44.650100
3503.982142	349514.149984	44.655105
3503.717857	349523.099768	44.660109
3503.987609	349517.941444	44.665114
3503.770532	349534.111942	44.670119
3503.774273	349525.661549	44.675124
3503.665061	349498.725889	44.680129
3503.626530	349491.325679	44.685133
3503.842014	349487.753915	44.690138
3503.724446	349492.379232	44.695143
3503.592798	349485.579123	44.700148
3504.019101	349488.285964	44.705153
3503.885361	349488.434402	44.710157
3504.081272	349484.280351	44.715162
3503.811404	349494.758103	44.720167
3503.867633	349489.938949	44.725172
3503.837926	349481.137518	44.730177
3503.573279	349484.335361	44.735181
3503.811752	349480.581803	44.740186
3503.921849	349469.111328	44.745191
3504.008467	349474.315200	44.750196
3504.034408	349476.958078	44.755201
3503.600118	349482.676972	44.760205
3503.931279	349472.673180	44.765210
3503.721328	349464.816489	44.770215
3503.676382	349443.826261	44.775220
3503.623023	349432.432522	44.780225
3503.613282	349445.668811	44.785229
3503.945018	349434.163291	44.790234
3504.060577	349442.136790	44.795239
3503.521170	349449.628449	44.800244
3504.103230	349449.434665	44.805249
3504.143245	349441.462101	44.810253
3504.244824	349420.219637	44.815258
3503.896047	349417.958737	44.820263
3504.129854	349428.204169	44.825268
3504.016339	349418.499728	44.830273
3503.824036	349397.761839	44.835277
3503.990640	349380.683108	44.840282
3503.854956	349385.667618	44.845287
3503.782940	349376.083866	44.850292
3504.073002	349383.622564	44.855297
3503.870427	349389.788413	44.860301
3504.171728	349375.258976	44.865306
3503.905635	349363.008055	44.870311
3504.011905	349351.665418	44.875316
3504.004726	349347.161692	44.880321
3503.930526	349348.446031	44.885325
3503.970452	349338.717318	44.890330
3503.971329	349338.386349	44.895335
3503.645105	349329.046387	44.900340
3503.633884	349324.365138	44.905345
3503.560785	349325.242081	44.910349
3503.497157	349317.438592	44.915354
3503.752637	349325.084571	44.920359
3503.521077	349335.479943	44.925364
3503.620425	349319.506236	44.930369
3503.735572	349331.882913	44.935373
3503.790985	349321.999040	44.940378
3503.562013	349336.033556	44.945383
3503.759069	349326.992641	44.950388
3503.959618	349333.451086	44.955393
3503.544670	349334.432974	44.960397
3503.678100	349323.518711	44.965402
3503.519789	349331.917294	44.970407
3503.871800	349323.080944	44.975412
3504.138326	349305.171947	44.980417
3503.618870	349308.893660	44.985421
3503.836958	349303.896192	44.990426
3503.503220	349306.570488	44.995431
3504.011660	349298.854719	45.000436
3503.608794	349309.251726	45.005441
3503.694533	349303.817056	45.010445
3504.166889	349304.785929	45.015450
3503.575766	349292.357312	45.020455
3503.730311	349277.800147	45.025460
3503.559865	349272.456877	45.030465
3503.422181	349272.911356	45.035469
3503.676724	349276.307099	45.040474
3503.721758	349268.919099	45.045479
3503.828038	349273.941722	45.050484
3503.966560	349280.511785	45.055489
3503.733890	349277.468981	45.060493
3503.958733	349284.916198	45.065498
3504.334641	349274.523525	45.070503
3503.720025	349263.040319	45.075508
3504.075118	349240.714199	45.080513
3503.881604	349247.642175	45.085517
3503.783488	349248.624879	45.090522
3503.856094	349252.380255	45.095527
3504.009724	349248.029259	45.100532
3503.482371	349243.556855	45.105537
3503.386225	349240.925141	45.110541
3503.705561	349240.645633	45.115546
3503.923200	349228.140049	45.120551
3503.620909	349216.556555	45.125556
3504.211272	349210.711232	45.130561
3503.725591	349218.067171	45.135565
3504.021607	349200.204382	45.140570
3504.084041	349220.632082	45.145575
3503.906365	349209.232499	45.150580
3503.826083	349202.093365	45.155585
3503.700277	349184.551770	45.160589
3503.757883	349180.165046	45.165594
3503.946422	349191.588446	45.170599
3503.715697	349186.229245	45.175604
3503.816525	349190.692805	45.180609
3503.987943	349187.738823	45.185613
3503.778362	349184.361495	45.190618
3503.782993	349167.002886	45.195623
3503.842422	349158.594536	45.200628
3503.812161	349150.633040	45.205633
3503.738579	349149.092169	45.210637
3504.283672	349152.620148	45.215642
3503.890218	349163.244757	45.220647
3503.643372	349160.891379	45.225652
3503.817070	349155.111919	45.230657
3503.720491	349147.466324	45.235661
3503.996673	349133.195310	45.240666
3503.428839	349133.361471	45.245671
3503.630402	349131.980714	45.250676
3503.728466	349131.812541	45.255681
3503.884113	349142.044930	45.260685
3504.017345	349128.280092	45.265690
3504.095017	349135.699692	45.270695
3503.639482	349137.069772	45.275700
3503.701524	349136.041942	45.280705
3503.803514	349120.474984	45.285709
3503.736449	349093.939689	45.290714
3503.665073	349111.105337	45.295719
3503.408944	349098.878234	45.300724
3503.686589	349102.550302	45.305729
3503.651956	349099.323472	45.310733
3503.743811	349099.741665	45.315738
3503.880262	349094.960697	45.320743
3503.647631	349113.907992	45.325748
3503.834493	349097.004131	45.330753
3503.616424	349109.637147	45.335757
3503.586966	349108.649233	45.340762
3503.827547	349113.039802	45.345767
3503.973062	349110.904361	45.350772
3504.110898	349087.645368	45.355777
3503.687911	349084.429028	45.360781
3503.901949	349067.928087	45.365786
3504.002311	349077.507488	45.370791
3503.859604	349085.572771	45.375796
3503.978325	349080.565541	45.380801
3503.843728	349071.933335	45.385805
3503.842134	349050.147107	45.390810
3503.741262	349045.225492	45.395815
3503.499558	349050.201341	45.400820
3503.876648	349041.793658	45.405825
3503.508801	349056.461036	45.410829
3503.907556	349041.687042	45.415834
3503.794592	349046.897055	45.420839
3503.690662	349046.608104	45.425844
3503.962649	349053.182547	45.430849
3503.716493	349054.824947	45.435853
3503.698367	349045.487133	45.440858
3503.400773	349048.206630	45.445863
3503.601836	349034.354691	45.450868
3503.552607	349032.453645	45.455873
3503.450744	349031.553531	45.460877
3503.547120	349035.203357	45.465882
3503.874928	349029.017748	45.470887
3503.770642	349039.978441	45.475892
3503.786005	349037.227283	45.480897
3503.752679	349035.171014	45.485901
3503.836688	349032.358101	45.490906
3503.559378	349033.954523	45.495911
3503.917652	349043.976737	45.500916
3503.791460	349037.099355	45.505921
3503.632629	349053.846170	45.510925
3503.885067	349043.422069	45.515930
3504.004232	349026.401632	45.520935
3503.700589	349018.127013	45.525940
3504.014347	349003.620961	45.530945
3503.543856	349008.123951	45.535949
3503.952889	348993.526480	45.540954
3503.857895	349015.608045	45.545959
3503.791764	349011.597191	45.550964
3503.849428	348998.302395	45.555969
3503.425964	349007.150169	45.560973
3503.509175	349001.766772	45.565978
3503.722142	348986.258587	45.570983
3503.467047	348986.324405	45.575988
3503.453688	348975.433279	45.580993
3503.454603	348979.454523	45.585997
3503.602790	348988.390089	45.591002
3503.400468	348986.615051	45.596007
3503.495831	349002.507245	45.601012
3503.941795	349005.032842	45.606017
3503.695306	348998.988922	45.611021
3504.024887	348981.298918	45.616026
3503.538439	348994.228903	45.621031
3503.836219	348988.811584	45.626036
3503.741652	348988.826572	45.631041
3503.850792	348993.925123	45.636045
3504.008375	348993.034896	45.641050
3503.785261	348991.263144	45.646055
3503.566053	348989.872548	45.651060
3503.492554	348968.046752	45.656065
3503.628958	348977.824085	45.661069
3503.742268	348960.855456	45.666074
3503.838366	348958.626014	45.671079
3503.775268	348963.879054	45.676084
3503.598299	348961.489169	45.681089
3503.391164	348963.227209	45.686093
3503.688612	348955.162974	45.691098
3503.924665	348970.193034	45.696103
3503.749128	348959.963834	45.701108
3503.948923	348954.332938	45.706113
3503.779453	348970.190654	45.711117
3503.873812	348969.335873	45.716122
3503.701962	348949.739905	45.721127
3503.663272	348953.920121	45.726132
3503.482363	348946.160571	45.731137
3503.443933	348941.127269	45.736141
3503.673534	348950.813519	45.741146
3503.581265	348953.016981	45.746151
3503.460063	348951.178214	45.751156
3503.794163	348944.278956	45.756161
3503.377101	348956.027208	45.761165
3503.655983	348945.853425	45.766170
3503.622192	348958.991826	45.771175
3503.714525	348949.865598	45.776180
3503.824224	348948.448457	45.781185
3503.567714	348958.847844	45.786189
3503.642306	348943.845103	45.791194
3503.555951	348952.206915	45.796199
3503.431856	348960.421983	45.801204
3503.852546	348948.953203	45.806209
3503.468816	348955.554964	45.811213
3504.193950	348948.364825	45.816218
3504.035753	348967.300402	45.821223
3503.726480	348937.316456	45.826228
3504.035295	348928.410517	45.831233
3503.889580	348928.433591	45.836237
3504.150444	348919.102555	45.841242
3503.956284	348933.309830	45.846247
3503.469016	348926.693129	45.851252
3503.837785	348918.923033	45.856257
3503.665004	348914.598161	45.861261
3503.747849	348894.020199	45.866266
3503.760142	348897.810585	45.871271
3503.941385	348898.240100	45.876276
3503.606794	348891.497452	45.881281
3503.638434	348892.434198	45.886285
3503.841956	348901.946418	45.891290
3504.003919	348900.088336	45.896295
3503.599029	348904.733673	45.901300
3503.859636	348903.979867	45.906305
3503.805077	348898.185563	45.911309
3503.656455	348877.415122	45.916314
3503.267253	348874.040720	45.921319
3503.648665	348873.573235	45.926324
3503.618181	348853.980336	45.931329
3503.650032	348873.496741	45.936333
3503.757348	348862.459258	45.941338
3503.699199	348874.074432	45.946343
3503.619471	348868.614974	45.951348
3504.049214	348876.818854	45.956353
3503.799835	348872.633347	45.961357
3504.033451	348871.196613	45.966362
3503.655308	348875.634112	45.971367
3503.627409	348875.434948	45.976372
3503.852583	348877.970003	45.981377
3503.566459	348866.460235	45.986381
3503.467897	348849.219647	45.991386
3503.571896	348852.028376	45.996391
3503.533890	348843.202704	46.001396
3503.757980	348846.119706	46.006401
3503.746290	348852.229986	46.011405
3503.722536	348851.419327	46.016410
3503.849736	348841.753085	46.021415
3503.884855	348862.617914	46.026420
3503.851890	348856.234804	46.031425
3503.672145	348861.200875	46.036429
3503.861964	348847.376118	46.041434
3504.027766	348846.001008	46.046439
3503.265059	348838.409774	46.051444
3503.790209	348813.562338	46.056449
3503.491927	348822.364900	46.061453
3503.739022	348817.515513	46.066458
3503.808901	348815.951954	46.071463
3503.822497	348826.588633	46.076468
3503.949215	348822.063697	46.081473
3503.852221	348829.536402	46.086477
3503.948924	348833.949739	46.091482
3503.845556	348823.989073	46.096487
3503.827808	348815.338355	46.101492
3503.640073	348798.391817	46.106497
3503.783294	348793.431591	46.111501
3503.816089	348798.287712	46.116506
3503.771435	348793.866221	46.121511
3503.743867	348791.274548	46.126516
3503.842586	348797.672799	46.131521
3503.492182	348792.841513	46.136525
3503.863270	348794.157276	46.141530
3503.757652	348790.127197	46.146535
3503.688589	348791.817963	46.151540
3503.787384	348789.282668	46.156545
3503.435353	348766.126435	46.161549
3503.897912	348771.856330	46.166554
3503.481629	348758.483692	46.171559
3503.395334	348770.536016	46.176564
3503.819017	348756.419749	46.181569
3503.560844	348761.780003	46.186573
3503.732492	348746.507348	46.191578
3504.091497	348756.682209	46.196583
3503.942044	348756.069582	46.201588
3504.100228	348764.978152	46.206593
3503.698739	348763.209140	46.211597
3503.734054	348754.168250	46.216602
3503.642422	348745.325588	46.221607
3503.668614	348737.507818	46.226612
3503.710901	348722.942803	46.231617
3503.732814	348743.657054	46.236621
3504.163349	348737.429721	46.241626
3504.129881	348744.408813	46.246631
3503.944792	348732.272204	46.251636
3503.942841	348716.696114	46.256641
3503.748066	348700.336047	46.261645
3504.086148	348689.923794	46.266650
3503.867273	348698.739273	46.271655
3503.764390	348713.873888	46.276660
3504.086834	348708.885321	46.281665
3504.008191	348708.083338	46.286669
3503.773168	348690.966080	46.291674
3503.953322	348682.334960	46.296679
3503.775169	348680.479735	46.301684
3503.474631	348675.691459	46.306689
3503.535283	348681.179480	46.311693
3503.824968	348667.237084	46.316698
3503.607421	348681.600831	46.321703
3503.560288	348684.713430	46.326708
3503.750993	348672.695562	46.331713
3503.993968	348672.199058	46.336717
3503.940177	348673.429282	46.341722
3503.760205	348662.360822	46.346727
3503.737408	348650.020377	46.351732
3504.073176	348650.043689	46.356737
3503.581381	348646.507329	46.361741
3503.738161	348651.242056	46.366746
3503.842571	348642.088417	46.371751
3503.497149	348658.686686	46.376756
3503.638631	348652.581395	46.381761
3503.461810	348655.638142	46.386765
3503.600125	348655.590863	46.391770
3503.762839	348650.703898	46.396775
3503.724918	348656.869249	46.401780
3504.191014	348655.981148	46.406785
3503.505323	348645.094439	46.411789
3503.708377	348632.005638	46.416794
3503.893378	348629.889387	46.421799
3503.570819	348630.118580	46.426804
3503.927369	348623.852028	46.431809
3503.989432	348632.241329	46.436813
3503.515837	348623.179063	46.441818
3503.883124	348630.883818	46.446823
3503.671469	348629.390212	46.451828
3503.694163	348640.101843	46.456833
3503.560084	348638.875943	46.461837
3503.682529	348626.334370	46.466842
3503.786598	348608.247218	46.471847
3503.291028	348607.282078	46.476852
3503.533611	348597.928426	46.481857
3503.404514	348597.974325	46.486861
3503.380923	348595.025690	46.491866
3503.697937	348608.974075	46.496871
3503.812272	348605.570955	46.501876
3504.108229	348596.616094	46.506881
3503.613394	348605.246148	46.511885
3503.879961	348598.612042	46.516890
3504.012450	348594.162530	46.521895
3503.876439	348605.942779	46.526900
3503.865585	348606.377213	46.531905
3503.861164	348589.503439	46.536909
3503.685333	348575.940034	46.541914
3503.470015	348569.916592	46.546919
3503.624216	348572.259267	46.551924
3504.246281	348563.736429	46.556929
3503.535503	348571.331653	46.561933
3503.875959	348579.371530	46.566938
3504.093786	348570.988954	46.571943
3503.486587	348567.801705	46.576948
3503.944462	348572.437936	46.581953
3503.831002	348562.020686	46.586957
3503.690948	348543.386716	46.591962
3503.865810	348540.253993	46.596967
3503.536400	348545.192849	46.601972
3503.994518	348528.042320	46.606977
3503.683173	348537.737803	46.611981
3503.618727	348533.064902	46.616986
3503.758940	348535.180724	46.621991
3503.459961	348538.740373	46.626996
3503.858212	348532.289056	46.632001
3503.491041	348535.223191	46.637005
3503.740791	348536.430884	46.642010
3503.812666	348547.592890	46.647015
3503.614594	348539.377865	46.652020
3503.518779	348514.195784	46.657025
3503.456744	348522.248395	46.662029
3503.691498	348527.276226	46.667034
3503.876096	348520.731425	46.672039
3503.615276	348506.163367	46.677044
3503.807826	348512.139589	46.682049
3503.783077	348515.986760	46.687053
3503.871731	348502.356074	46.692058
3503.774044	348521.587659	46.697063
3503.645992	348519.419087	46.702068
3503.771261	348512.680049	46.707073
3503.552823	348525.873194	46.712077
3503.318193	348515.093315	46.717082
3503.970202	348521.047804	46.722087
3503.806397	348532.730656	46.727092
3503.932144	348501.328759	46.732097
3503.839206	348493.835209	46.737101
3503.630247	348476.917380	46.742106
3503.629444	348481.651581	46.747111
3503.500120	348495.899621	46.752116
3503.830288	348477.318551	46.757121
3503.568557	348489.958609	46.762125
3503.230806	348486.117917	46.767130
3503.503093	348484.675060	46.772135
3503.496855	348493.864185	46.777140
3503.562207	348492.861272	46.782145
3503.402544	348494.490015	46.787149
3503.487069	348491.524282	46.792154
3503.400840	348485.836748	46.797159
3503.330719	348494.170611	46.802164
3503.934512	348491.911794	46.807169
3503.732094	348502.251810	46.812173
3503.664493	348496.688592	46.817178
3503.970611	348498.167345	46.822183
3503.874318	348497.648118	46.827188
3503.928795	348501.151892	46.832193
3503.759294	348503.825713	46.837197
3504.034799	348478.610366	46.842202
3503.839865	348468.791371	46.847207
3503.650841	348465.767074	46.852212
3503.799649	348463.681991	46.857217
3503.630838	348477.910827	46.862221
3503.433658	348475.905892	46.867226
3503.727438	348468.987499	46.872231
3503.522681	348473.423070	46.877236
3503.401913	348476.598225	46.882241
3503.576027	348475.858087	46.887245
3503.428503	348477.993947	46.892250
3503.507803	348470.345907	46.897255
3503.446209	348482.139869	46.902260
3503.727931	348482.782569	46.907265
3503.579869	348480.693515	46.912269
3503.536600	348477.951598	46.917274
3503.658484	348490.200138	46.922279
3503.653266	348485.874195	46.927284
3503.802578	348483.025478	46.932289
3503.507274	348489.206085	46.937293
3503.730494	348487.770986	46.942298
3504.075956	348478.146532	46.947303
3503.384163	348456.978220	46.952308
3503.321195	348455.104779	46.957313
3503.525039	348466.016872	46.962317
3503.261834	348465.142255	46.967322
3503.547329	348484.007854	46.972327
3503.714891	348490.675227	46.977332
3503.838479	348471.363258	46.982337
3503.589605	348468.933815	46.987341
3503.522075	348460.112750	46.992346
3503.882116	348464.306323	46.997351
3503.793975	348458.364571	47.002356
3503.955165	348455.157650	47.007361
3503.631350	348454.139903	47.012365
3503.560885	348461.735722	47.017370
3503.799474	348467.882833	47.022375
3503.638857	348472.845914	47.027380
3503.655833	348460.091911	47.032385
3503.577690	348474.280962	47.037389
3503.810748	348471.800783	47.042394
3503.802719	348467.322572	47.047399
3503.381385	348453.416172	47.052404
3503.717789	348432.314371	47.057409
3503.779571	348437.980399	47.062413
3503.796976	348435.916088	47.067418
3503.583435	348435.389945	47.072423
3503.611501	348436.072746	47.077428
3503.752365	348432.792681	47.082433
3503.679867	348430.869842	47.087437
3503.955221	348431.080868	47.092442
3504.066756	348441.371264	47.097447
3503.628389	348437.521022	47.102452
3503.548737	348435.726572	47.107457
3503.747667	348447.784778	47.112461
3503.884053	348422.311429	47.117466
3503.693790	348407.935806	47.122471
3503.565369	348408.846961	47.127476
3503.770321	348400.440943	47.132481
3503.612927	348408.712260	47.137485
3503.422093	348407.800749	47.142490
3503.984114	348401.425334	47.147495
3503.744800	348407.189869	47.152500
3504.105799	348404.893076	47.157505
3503.886516	348404.876876	47.162509
3504.079288	348394.767510	47.167514
3503.867763	348381.107894	47.172519
3503.807219	348382.491903	47.177524
3503.823216	348364.291337	47.182529
3503.653771	348381.370905	47.187533
3503.699632	348374.618952	47.192538
3504.046942	348372.273418	47.197543
3503.972399	348382.898664	47.202548
3503.825814	348360.931472	47.207553
3503.645195	348344.543612	47.212557
3503.732030	348326.739064	47.217562
3503.775628	348332.866112	47.222567
3503.523365	348334.942180	47.227572
3503.992585	348334.359003	47.232577
3503.710319	348340.944795	47.237581
3503.821793	348327.386814	47.242586
3504.111450	348335.536564	47.247591
3503.735122	348332.185545	47.252596
3503.955133	348315.454371	47.257601
3503.970156	348313.848565	47.262605
3503.986578	348306.973999	47.267610
3503.867212	348309.283577	47.272615
3503.689845	348309.388011	47.277620
3503.793591	348312.578585	47.282625
3503.906373	348310.270125	47.287629
3503.616953	348304.385628	47.292634
3503.949439	348274.732553	47.297639
3503.527908	348283.172905	47.302644
3503.663845	348277.908362	47.307649
3503.524885	348270.218443	47.312653
3503.626494	348277.278046	47.317658
3503.817611	348278.495014	47.322663
3503.697855	348282.026346	47.327668
3503.654346	348267.678391	47.332673
3503.817990	348278.393262	47.337677
3503.798877	348277.480053	47.342682
3504.029603	348277.901751	47.347687
3503.592010	348282.959539	47.352692
3503.570768	348269.524333	47.357697
3503.538915	348263.344594	47.362701
3503.819490	348251.236073	47.367706
3503.600766	348239.664617	47.372711
3503.334782	348256.861292	47.377716
3503.550436	348242.319649	47.382721
3503.529945	348243.493715	47.387725
3503.462517	348242.079106	47.392730
3503.801527	348247.268645	47.397735
3503.223720	348254.359303	47.402740
3503.695025	348242.424242	47.407745
3503.588257	348243.917371	47.412749
3503.722019	348253.288018	47.417754
3503.667469	348251.260527	47.422759
3503.419872	348251.936006	47.427764
3503.790119	348252.004772	47.432769
3503.818807	348256.785234	47.437773
3503.732700	348260.362152	47.442778
3503.763025	348268.960139	47.447783
3503.502798	348257.904286	47.452788
3503.562252	348250.717487	47.457793
3503.768793	348263.843510	47.462797
3503.564838	348270.213315	47.467802
3503.709990	348259.806030	47.472807
3503.741374	348274.359595	47.477812
3503.842705	348255.381946	47.482817
3503.548816	348246.189401	47.487821
3503.597534	348232.590415	47.492826
3503.583147	348228.927651	47.497831
3503.842115	348231.915528	47.502836
3504.038264	348216.689760	47.507841
3503.649416	348235.458433	47.512845
3503.632428	348225.025870	47.517850
3504.052601	348226.308436	47.522855
3503.761099	348246.257956	47.527860
3503.719708	348231.222456	47.532865
3503.916541	348233.227530	47.537869
3503.559346	348219.158221	47.542874
3503.590804	348207.139976	47.547879
3503.556420	348209.207056	47.552884
3503.917955	348201.056226	47.557889
3503.590676	348215.997382	47.562893
3503.764394	348207.036331	47.567898
3503.750183	348204.366163	47.572903
3503.287301	348208.053552	47.577908
3503.569279	348210.197879	47.582913
3503.590036	348211.874463	47.587917
3503.482020	348210.848048	47.592922
3503.663959	348224.079777	47.597927
3503.389910	348220.738034	47.602932
3503.699890	348211.322759	47.607937
3503.873001	348226.592038	47.612941
3503.650321	348224.794741	47.617946
3503.862909	348221.197902	47.622951
3503.553942	348220.992265	47.627956
3503.758462	348220.170962	47.632961
3503.715530	348232.038382	47.637965
3503.683875	348221.150003	47.642970
3503.854754	348191.293365	47.647975
3503.676933	348194.604814	47.652980
3503.717847	348186.530120	47.657985
3503.578139	348183.752531	47.662989
3503.411798	348189.200129	47.667994
3503.762446	348184.945164	47.672999
3503.381310	348184.470965	47.678004
3503.458174	348185.553285	47.683009
3503.503457	348196.057815	47.688013
3503.754609	348196.399929	47.693018
3503.780423	348200.493647	47.698023
3503.478979	348199.599619	47.703028
3503.858177	348194.296612	47.708033
3503.737648	348201.518602	47.713037
3503.805347	348195.068598	47.718042
3503.980663	348193.768325	47.723047
3503.759885	348185.938617	47.728052
3503.597151	348168.911579	47.733057
3503.327503	348161.420469	47.738061
3503.528872	348156.552802	47.743066
3503.733190	348156.036953	47.748071
3503.665266	348156.633124	47.753076
3503.677501	348159.252779	47.758081
3503.829223	348161.570412	47.763085
3503.684459	348166.454658	47.768090
3503.950958	348164.961805	47.773095
3503.780795	348172.420713	47.778100
3503.940274	348158.575131	47.783105
3503.697610	348175.717241	47.788109
3503.619487	348169.086672	47.793114
3503.849007	348168.185059	47.798119
3503.657782	348153.376840	47.803124
3503.907417	348133.968474	47.808129
3503.802446	348137.777449	47.813133
3503.812744	348138.921198	47.818138
3504.004831	348126.699379	47.823143
3503.594482	348134.578042	47.828148
3503.866774	348137.538365	47.833153
3503.609135	348142.720430	47.838157
3503.717077	348135.144171	47.843162
3503.825738	348147.267616	47.848167
3503.672442	348124.130603	47.853172
3503.632188	348108.000455	47.858177
3503.726493	348107.858325	47.863181
3503.470395	348106.295375	47.868186
3503.847161	348104.046981	47.873191
3503.823731	348119.754591	47.878196
3503.792185	348102.401370	47.883201
3503.621849	348103.191896	47.888205
3503.774786	348115.639224	47.893210
3503.821731	348105.985543	47.898215
3503.685573	348114.838942	47.903220
3504.254553	348092.249483	47.908225
3503.855963	348084.829651	47.913229
3503.306529	348077.280952	47.918234
3503.633659	348067.710230	47.923239
3503.556998	348066.424336	47.928244
3503.617965	348072.065078	47.933249
3503.554417	348069.809936	47.938253
3503.080355	348071.539297	47.943258
3503.406254	348074.542054	47.948263
3502.927316	348089.329055	47.953268
3503.597080	348088.536008	47.958273
3503.527284	348113.388211	47.963277
3503.771283	348118.898206	47.968282
3504.207294	348101.852849	47.973287
3503.568296	348100.859470	47.978292
3503.901311	348084.263075	47.983297
3503.923937	348087.517390	47.988301
3503.904669	348092.509063	47.993306
3504.067611	348088.538285	47.998311
3503.825382	348082.340881	48.003316
3503.866740	348062.252760	48.008321
3503.689138	348057.674063	48.013325
3503.488442	348049.026697	48.018330
3503.609884	348052.494461	48.023335
3503.712399	348050.620297	48.028340
3503.529085	348047.136939	48.033345
3503.749494	348050.589058	48.038349
3503.795801	348049.461887	48.043354
3504.052515	348051.457502	48.048359
3503.683332	348054.290172	48.053364
3503.779996	348049.311789	48.058369
3503.881496	348057.796749	48.063373
3503.545503	348031.761600	48.068378
3504.066650	348028.726818	48.073383
3503.758842	348016.685811	48.078388
3503.677276	348022.832680	48.083393
3503.529521	348024.688621	48.088397
3503.646876	348024.899175	48.093402
3503.838001	348014.764549	48.098407
3503.434133	348013.454025	48.103412
3504.088812	348020.400775	48.108417
3503.711082	348030.514073	48.113421
3503.572941	348027.252640	48.118426
3503.921128	348020.427399	48.123431
3503.774591	348016.658253	48.128436
3503.959053	347992.678777	48.133441
3503.333783	347988.527175	48.138445
3503.529335	347980.504361	48.143450
3503.993429	347980.125607	48.148455
3503.534718	347991.982452	48.153460
3503.612834	347989.908527	48.158465
3503.672111	347991.808096	48.163469
3503.621127	347986.267652	48.168474
3503.551577	347986.176878	48.173479
3503.763838	347989.375768	48.178484
3503.893282	347995.209309	48.183489
3503.584194	347995.818155	48.188493
3503.942273	348002.353659	48.193498
3504.171389	347984.424702	48.198503
3503.633866	347958.828612	48.203508
3503.350845	347961.520405	48.208513
3503.744650	347955.502409	48.213517
3503.564809	347952.425729	48.218522
3503.884161	347952.120761	48.223527
3503.875327	347958.943343	48.228532
3504.073500	347946.949592	48.233537
3503.864715	347951.818526	48.238541
3503.744169	347951.506744	48.243546
3503.844629	347920.617561	48.248551
3503.664528	347929.274319	48.253556
3503.896539	347929.008610	48.258561
3503.674342	347927.109419	48.263565
3503.782717	347922.027365	48.268570
3503.944435	347916.758713	48.273575
3503.541252	347920.080354	48.278580
3503.856626	347920.132344	48.283585
3503.716235	347930.360851	48.288589
3503.385372	347931.202209	48.293594
3503.891750	347917.785316	48.298599
3503.205488	347918.479242	48.303604
3503.609202	347925.796555	48.308609
3503.472238	347925.792794	48.313613
3503.706546	347930.235353	48.318618
3503.708826	347918.959769	48.323623
3503.513523	347917.259942	48.328628
3503.692311	347898.728065	48.333633
3503.550748	347902.542841	48.338637
3503.689213	347897.226959	48.343642
3503.633772	347896.548556	48.348647
3503.198849	347908.274398	48.353652
3503.471992	347895.454317	48.358657
3503.520366	347901.275232	48.363661
3503.500791	347899.802145	48.368666
3503.668730	347892.038205	48.373671
3503.499466	347909.474217	48.378676
3503.754872	347897.700475	48.383681
3503.856728	347905.014607	48.388685
3503.448097	347907.140862	48.393690
3503.844763	347901.198765	48.398695
3503.797765	347901.588014	48.403700
3503.628933	347906.399732	48.408705
3503.727165	347903.457253	48.413709
3503.717012	347911.018160	48.418714
3503.994268	347902.676994	48.423719
3503.625048	347913.756146	48.428724
3503.686291	347910.157761	48.433729
3503.386876	347894.221235	48.438733
3503.311670	347914.671172	48.443738
3503.766295	347909.737996	48.448743
3503.388818	347906.870721	48.453748
3503.414532	347921.196206	48.458753
3503.632147	347914.391593	48.463757
3503.659688	347911.460291	48.468762
3504.232108	347904.446874	48.473767
3503.545172	347903.639235	48.478772
3503.822386	347881.503050	48.483777
3503.662563	347884.633508	48.488781
3503.352594	347885.318851	48.493786
3503.548200	347884.142622	48.498791
3503.583317	347884.849767	48.503796
3503.769234	347875.046816	48.508801
3503.486789	347891.355383	48.513805
3503.518898	347884.020148	48.518810
3503.737774	347875.306426	48.523815
3503.470324	347887.794810	48.528820
3503.827805	347873.816049	48.533825
3503.714266	347885.567444	48.538829
3503.981930	347886.721416	48.543834
3504.113670	347869.545926	48.548839
3503.747222	347866.346029	48.553844
3503.842458	347853.452256	48.558849
3503.728784	347847.768996	48.563853
3503.712684	347856.781620	48.568858
3503.712799	347843.113867	48.573863
3503.401247	347861.946801	48.578868
3503.840734	347839.632233	48.583873
3503.615799	347854.480949	48.588877
3502.922046	347853.928908	48.593882
3503.572496	347848.379370	48.598887
3503.600419	347858.097692	48.603892
3503.568844	347857.797297	48.608897
3503.724859	347859.910647	48.613901
3504.224828	347852.425088	48.618906
3504.178896	347847.418326	48.623911
3503.626110	347828.569393	48.628916
3503.846703	347811.583456	48.633921
3503.916293	347821.167937	48.638925
3503.521796	347818.888747	48.643930
3503.445501	347817.679146	48.648935
3503.686869	347823.393202	48.653940
3503.699847	347826.776319	48.658945
3503.640353	347827.829299	48.663949
3503.890958	347822.699299	48.668954
3503.802629	347817.673784	48.673959
3503.300198	347828.366778	48.678964
3503.622875	347815.462492	48.683969
3503.674903	347819.526643	48.688973
3503.620080	347828.621749	48.693978
3503.752762	347827.659084	48.698983
3503.427305	347810.861279	48.703988
3503.490754	347815.890805	48.708993
3503.496885	347823.347340	48.713997
3503.492403	347826.096915	48.719002
3504.013477	347816.240969	48.724007
3503.433255	347803.683035	48.729012
3503.380326	347795.419504	48.734017
3503.468098	347796.983698	48.739021
3503.312200	347805.509388	48.744026
3503.411271	347816.412719	48.749031
3503.442689	347820.836457	48.754036
3503.459875	347829.182068	48.759041
3503.490092	347839.205456	48.764045
3503.525751	347843.501261	48.769050
3503.754641	347842.294318	48.774055
3503.737448	347850.441745	48.779060
3503.867626	347828.074263	48.784065
3503.862525	347810.971293	48.789069
3503.589147	347806.611334	48.794074
3503.567477	347795.084990	48.799079
3503.531694	347807.460413	48.804084
3503.805489	347804.362914	48.809089
3503.685573	347801.836698	48.814093
3503.795499	347816.454322	48.819098
3504.075775	347809.207105	48.824103
3503.820761	347804.742435	48.829108
3503.757050	347807.145043	48.834113
3503.643699	347810.420871	48.839117
3503.721479	347796.257239	48.844122
3503.639130	347774.610541	48.849127
3503.302296	347785.760955	48.854132
3503.467047	347787.236623	48.859137
3503.710599	347787.121802	48.864141
3503.766218	347778.815656	48.869146
3504.300076	347777.942282	48.874151
3503.787705	347784.793584	48.879156
3503.684549	347783.333708	48.884161
3503.661833	347789.140421	48.889165
3503.579838	347792.156771	48.894170
3503.766817	347790.192889	48.899175
3503.436669	347793.732060	48.904180
3503.663710	347790.285622	48.909185
3503.764882	347798.007110	48.914189
3503.635482	347788.432157	48.919194
3503.459080	347758.095696	48.924199
3503.388997	347753.143647	48.929204
3503.743077	347763.217659	48.934209
3503.659733	347758.827654	48.939213
3503.550176	347762.026529	48.944218
3503.515031	347760.835873	48.949223
3503.588950	347754.410288	48.954228
3503.544493	347750.319560	48.959233
3503.589654	347756.599137	48.964237
3503.485562	347760.967946	48.969242
3503.426198	347754.894309	48.974247
3503.541360	347764.726116	48.979252
3503.571307	347760.038228	48.984257
3503.579997	347770.548623	48.989261
3503.674090	347766.945036	48.994266
3503.720767	347767.777615	48.999271
3503.455934	347769.372101	49.004276
3503.457751	347765.095894	49.009281
3503.600451	347771.003719	49.014285
3503.497534	347773.590692	49.019290
3503.773543	347770.289224	49.024295
3503.587145	347775.256443	49.029300
3503.557066	347767.651050	49.034305
3504.047088	347767.675430	49.039309
3503.924938	347778.613741	49.044314
3504.204236	347765.919919	49.049319
3503.845415	347756.203064	49.054324
3503.979764	347734.445737	49.059329
3503.639271	347745.469476	49.064333
3503.609750	347741.427291	49.069338
3503.926879	347735.039612	49.074343
3503.945473	347746.922860	49.079348
3504.009871	347741.695030	49.084353
3503.780605	347737.277187	49.089357
3503.557849	347719.215965	49.094362
3503.759243	347702.971143	49.099367
3503.537399	347718.175736	49.104372
3503.575372	347699.436985	49.109377
3503.710234	347700.841024	49.114381
3503.532645	347704.432440	49.119386
3503.908503	347693.479535	49.124391
3503.886039	347706.463726	49.129396
3503.711599	347691.423662	49.134401
3503.630503	347696.857832	49.139405
3503.837740	347700.108437	49.144410
3504.052483	347692.617044	49.149415
3503.822332	347711.589872	49.154420
3503.642154	347676.265341	49.159425
3503.863428	347672.107147	49.164429
3503.532927	347676.180877	49.169434
3503.549445	347667.270044	49.174439
3503.721404	347675.463949	49.179444
3503.822811	347672.750026	49.184449
3503.592482	347665.532607	49.189453
3503.605238	347669.882951	49.194458
3503.961690	347660.612951	49.199463
3503.872647	347678.087256	49.204468
3503.936658	347665.885585	49.209473
3503.734908	347645.606679	49.214477
3503.381053	347639.706847	49.219482
3503.523820	347632.914033	49.224487
3503.470034	347630.988208	49.229492
3503.921917	347628.320685	49.234497
3503.778837	347645.141787	49.239501
3503.370619	347637.825226	49.244506
3503.602347	347632.316410	49.249511
3503.353958	347634.824578	49.254516
3503.858609	347641.031527	49.259521
3503.449907	347636.336618	49.264525
3503.328871	347637.399330	49.269530
3503.539438	347640.013108	49.274535
3503.536043	347631.665365	49.279540
3503.639852	347637.910231	49.284545
3503.714284	347631.968143	49.289549
3503.926554	347638.933975	49.294554
3503.939036	347641.808137	49.299559
3503.857528	347641.566539	49.304564
3503.695782	347643.831940	49.309569
3503.786545	347640.865176	49.314573
3503.537387	347648.947494	49.319578
3503.667767	347636.353541	49.324583
3503.330811	347638.239406	49.329588
3503.969286	347625.005179	49.334593
3503.679759	347620.545950	49.339597
3503.292773	347611.927967	49.344602
3503.530478	347610.592365	49.349607
3503.330393	347618.030624	49.354612
3503.418291	347615.624260	49.359617
3503.559088	347622.525037	49.364621
3503.439269	347628.041691	49.369626
3503.555292	347620.820417	49.374631
3503.439053	347623.434955	49.379636
3503.664834	347631.976688	49.384641
3503.732752	347630.235241	49.389645
3503.349260	347628.921487	49.394650
3504.004899	347613.622916	49.399655
3503.527522	347631.082270	49.404660
3503.633973	347617.575818	49.409665
3503.645808	347625.209643	49.414669
3503.612898	347618.113722	49.419674
3503.545747	347627.618045	49.424679
3503.369628	347627.722282	49.429684
3503.666877	347626.886311	49.434689
3503.924988	347633.692184	49.439693
3503.785571	347622.286229	49.444698
3504.130800	347624.980527	49.449703
3504.015589	347625.406014	49.454708
3503.637212	347605.002303	49.459713
3503.406821	347597.250389	49.464717
3503.537600	347594.760889	49.469722
3503.551930	347589.795481	49.474727
3503.596872	347601.445525	49.479732
3503.634514	347592.658602	49.484737
3503.436646	347591.697285	49.489741
3503.391979	347601.783458	49.494746
3503.903850	347592.641590	49.499751
3503.688786	347598.835061	49.504756
3503.654838	347602.760106	49.509761
3503.785899	347597.954411	49.514765
3503.806394	347586.166837	49.519770
3504.171668	347596.290013	49.524775
3503.681901	347606.064767	49.529780
3503.803077	347586.625616	49.534785
3504.068258	347588.390839	49.539789
3503.734518	347581.622446	49.544794
3504.074916	347555.098364	49.549799
3503.844520	347565.621140	49.554804
3503.689117	347562.056983	49.559809
3503.696836	347568.367952	49.564813
3503.904778	347555.430841	49.569818
3503.816739	347564.454884	49.574823
3503.632531	347573.035988	49.579828
3503.818677	347555.953612	49.584833
3503.938044	347533.587723	49.589837
3503.650705	347532.742358	49.594842
3503.765976	347513.431376	49.599847
3503.892479	347521.199802	49.604852
3503.544749	347524.919935	49.609857
3503.480643	347529.180631	49.614861
3503.382981	347519.396997	49.619866
3503.647148	347513.246735	49.624871
3503.378775	347527.135219	49.629876
3503.643068	347522.053932	49.634881
3503.797700	347521.851359	49.639885
3503.543141	347521.738927	49.644890
3503.995730	347533.120923	49.649895
3503.838470	347536.149186	49.654900
3503.955984	347519.739406	49.659905
3503.656241	347505.559027	49.664909
3503.971678	347506.145504	49.669914
3503.855735	347488.779985	49.674919
3503.728428	347505.013233	49.679924
3503.801491	347489.806727	49.684929
3503.804216	347494.235027	49.689933
3503.777216	347509.052542	49.694938
3503.979903	347490.847632	49.699943
3503.834651	347476.311942	49.704948
3503.595246	347465.838044	49.709953
3503.496975	347467.686181	49.714957
3503.287174	347462.756194	49.719962
3503.430655	347466.220510	49.724967
3503.179116	347469.721822	49.729972
3503.606472	347478.384426	49.734977
3503.620630	347466.750542	49.739981
3503.339690	347484.560672	49.744986
3503.600253	347477.571052	49.749991
3503.492027	347483.162244	49.754996
3503.577641	347486.737515	49.760001
3503.689270	347474.833702	49.765005
3503.555939	347476.254693	49.770010
3504.073338	347466.297459	49.775015
3503.447931	347470.545086	49.780020
3503.674274	347459.335798	49.785025
3503.927643	347463.877189	49.790029
3503.517896	347471.475874	49.795034
3503.454458	347465.275589	49.800039
3503.432859	347473.169243	49.805044
3503.537844	347472.592735	49.810049
3503.616972	347475.914510	49.815053
3503.456193	347485.535467	49.820058
3503.967396	347466.696374	49.825063
3503.596451	347479.761160	49.830068
3503.664053	347465.268175	49.835073
3503.919555	347469.096565	49.840077
3503.880505	347487.682926	49.845082
3503.726520	347460.549745	49.850087
3503.557306	347452.711784	49.855092
3503.821099	347442.718281	49.860097
3503.741960	347436.367761	49.865101
3503.574230	347445.811657	49.870106
3503.939653	347445.626665	49.875111
3503.669477	347442.716951	49.880116
3503.679876	347441.188209	49.885121
3503.740917	347435.375479	49.890125
3503.518768	347449.154865	49.895130
3503.682334	347446.125677	49.900135
3503.648979	347448.523502	49.905140
3503.460070	347450.996823	49.910145
3503.693394	347443.069771	49.915149
3503.372790	347454.828538	49.920154
3503.912903	347438.173761	49.925159
3503.830799	347445.135250	49.930164
3503.943080	347427.835442	49.935169
3504.237469	347421.884011	49.940173
3503.836344	347420.827562	49.945178
3503.729663	347401.398917	49.950183
3503.813050	347407.087086	49.955188
3503.805871	347412.662311	49.960193
3503.906110	347407.937829	49.965197
3503.571165	347394.806530	49.970202
3503.671147	347378.501291	49.975207
3503.601421	347377.417903	49.980212
3503.693024	347373.178377	49.985217
3503.928361	347380.471475	49.990221
3503.609587	347381.896332	49.995226
3504.106358	347374.843906	50.000231
3503.672602	347381.021069	50.005236
3503.506345	347378.782135	50.010241
3503.549347	347379.513493	50.015245
3503.394708	347381.090568	50.020250
3503.811543	347371.047406	50.025255
3503.535239	347384.351775	50.030260
3503.828640	347376.746096	50.035265
3503.674782	347378.399405	50.040269
3503.525041	347376.336027	50.045274
3503.763125	347385.766683	50.050279
3503.810726	347380.159690	50.055284
3503.638239	347364.050235	50.060289
3503.536385	347356.837918	50.065293
3503.584209	347365.382373	50.070298
3503.552793	347343.422031	50.075303
3503.428695	347349.753862	50.080308
3503.445352	347342.522809	50.085313
3503.520166	347344.190873	50.090317
3503.468863	347346.693349	50.095322
3503.619085	347346.873258	50.100327
3503.406311	347356.527908	50.105332
3503.321703	347347.123966	50.110337
3503.829730	347353.254056	50.115341
3503.460495	347346.720316	50.120346
3503.639955	347347.328292	50.125351
3503.378436	347345.791630	50.130356
3503.277629	347356.523029	50.135361
3503.534457	347348.261368	50.140365
3503.189606	347357.071520	50.145370
3503.513732	347369.059260	50.150375
3503.596952	347395.160204	50.155380
3504.053937	347385.390673	50.160385
3503.917304	347362.836117	50.165389
3503.556713	347362.104139	50.170394
3503.929806	347351.558842	50.175399
3503.953982	347364.433929	50.180404
3503.781273	347351.811471	50.185409
3504.055047	347351.895490	50.190413
3503.781527	347346.491973	50.195418
3503.537787	347332.506315	50.200423
3503.611094	347335.829019	50.205428
3504.147860	347327.395839	50.210433
3504.261556	347319.920371	50.215437
3503.606822	347324.503525	50.220442
3503.751622	347329.749304	50.225447
3503.881028	347336.270132	50.230452
3503.768866	347333.335432	50.235457
3504.035158	347300.027176	50.240461
3503.472819	347300.065209	50.245466
3503.657949	347280.743104	50.250471
3503.477836	347298.868233	50.255476
3503.776075	347291.490848	50.260481
3503.832480	347287.664118	50.265485
3503.577333	347288.442611	50.270490
3503.713874	347287.301160	50.275495
3503.508177	347293.162303	50.280500
3503.448784	347291.542781	50.285505
3503.395229	347287.377102	50.290509
3503.436773	347292.206518	50.295514
3503.538923	347297.815374	50.300519
3503.586482	347308.650590	50.305524
3503.781021	347297.751726	50.310529
3503.590331	347297.883719	50.315533
3503.493216	347298.611776	50.320538
3503.639880	347290.952926	50.325543
3503.581394	347300.557743	50.330548
3503.566881	347295.825941	50.335553
3503.442631	347294.827528	50.340557
3503.542668	347297.967841	50.345562
3503.531579	347301.278437	50.350567
3503.566045	347304.861806	50.355572
3503.960908	347294.720295	50.360577
3504.023752	347288.067337	50.365581
3503.421203	347289.180725	50.370586
3503.543892	347292.648339	50.375591
3503.521117	347297.284304	50.380596
3503.752283	347301.447433	50.385601
3503.903458	347285.694026	50.390605
3503.464036	347273.368238	50.395610
3503.726510	347269.152597	50.400615
3503.458544	347274.234563	50.405620
3503.874114	347279.335731	50.410625
3503.948899	347270.339267	50.415629
3504.023142	347272.872804	50.420634
3504.108201	347264.689190	50.425639
3503.672744	347263.994499	50.430644
3503.972529	347246.715898	50.435649
3503.591940	347236.595157	50.440653
3503.510521	347240.629541	50.445658
3503.978536	347228.007574	50.450663
3503.724128	347235.225399	50.455668
3503.693650	347240.193467	50.460673
3504.220646	347235.223339	50.465677
3503.693572	347242.306103	50.470682
3503.775703	347234.148400	50.475687
3503.694703	347229.987055	50.480692
3503.671050	347206.345576	50.485697
3503.769583	347202.944871	50.490701
3503.490629	347199.476580	50.495706
3503.926494	347186.426996	50.500711
3503.514047	347202.527240	50.505716
3503.615638	347199.533289	50.510721
3503.940272	347179.883668	50.515725
3503.586288	347196.229196	50.520730
3503.682792	347182.673308	50.525735
3503.430501	347151.406781	50.530740
3503.264954	347117.224948	50.535745
3503.217292	347104.760834	50.540749
3502.900371	347062.432669	50.545754
3502.982026	346995.148948	50.550759
3502.636998	346934.932040	50.555764
3502.409569	346866.628025	50.560769
3502.561220	346801.012876	50.565773
3502.058727	346718.575091	50.570778
3501.677109	346625.606140	50.575783
3501.439765	346540.199127	50.580788
3500.968526	346430.572522	50.585793
3501.058257	346318.922614	50.590797
3500.515449	346206.863431	50.595802
3500.207764	346089.447210	50.600807
3499.689897	345964.173569	50.605812
3498.956926	345835.981118	50.610817
3498.787027	345708.870206	50.615821
3498.203259	345575.104828	50.620826
3497.925537	345437.498238	50.625831
3496.991589	345300.122334	50.630836
3496.461016	345151.915598	50.635841
3495.935709	345010.223712	50.640845
3495.659817	344878.673416	50.645850
3495.542637	344718.309864	50.650855
3494.828424	344567.407165	50.655860
3494.027982	344413.616003	50.660865
3493.899071	344249.613169	50.665869
3493.033911	344092.471520	50.670874
3493.064059	343922.435554	50.675879
3492.182796	343756.946714	50.680884
3491.423879	343584.361875	50.685889
3491.308987	343404.165782	50.690893
3490.406357	343242.726093	50.695898
3489.876709	343058.521880	50.700903
3489.185647	342893.382406	50.705908
3488.268320	342718.961973	50.710913
3487.800519	342549.408122	50.715917
3487.124267	342380.115845	50.720922
3486.721725	342196.728922	50.725927
3486.038162	342015.218609	50.730932
3485.404982	341838.001638	50.735937
3485.012966	341643.716790	50.740941
3484.271333	341470.843220	50.745946
3483.824773	341276.693116	50.750951
3483.229928	341103.769861	50.755956
3482.370196	340921.520539	50.760961
3481.609775	340728.640190	50.765965
3481.000398	340545.001068	50.770970
3480.711264	340357.365207	50.775975
3479.757184	340183.936189	50.780980
3478.920943	339996.996682	50.785985
3478.858662	339792.548141	50.790989
3477.758863	339613.184005	50.795994
3477.365616	339426.478249	50.800999
3476.637078	339226.282500	50.806004
3475.885093	339038.945024	50.811009
3475.155247	338859.011167	50.816013
3474.431225	338667.111583	50.821018
3474.344081	338461.924506	50.826023
3473.355878	338279.815208	50.831028
3472.551199	338092.992445	50.836033
3472.050418	337887.232547	50.841037
3471.041989	337694.229526	50.846042
3470.408665	337500.988438	50.851047
3469.824307	337326.144087	50.856052
3469.083211	337134.344527	50.861057
3468.400899	336945.437175	50.866061
3467.737694	336757.188140	50.871066
3467.254002	336558.320170	50.876071
3466.613735	336384.449539	50.881076
3465.932764	336194.165180	50.886081
3465.388905	335997.672554	50.891085
3464.562995	335812.246862	50.896090
3463.917746	335603.753385	50.901095
3463.239228	335429.300828	50.906100
3462.544560	335241.536222	50.911105
3461.821669	335038.602979	50.916109
3461.114586	334851.399328	50.921114
3460.765497	334659.607132	50.926119
3459.872073	334473.246555	50.931124
3459.267848	334280.729920	50.936129
3458.718139	334089.375187	50.941133
3457.708175	333900.765765	50.946138
3457.357744	333707.876471	50.951143
3456.446380	333515.991819	50.956148
3456.147644	333314.055711	50.961153
3455.281589	333125.956074	50.966157
3454.275533	332934.619435	50.971162
3454.022103	332738.988139	50.976167
3453.127086	332550.713353	50.981172
3452.419776	332359.531603	50.986177
3452.276109	332172.664529	50.991181
3451.345838	331987.448848	50.996186
3450.435874	331783.441088	51.001191
3449.963867	331593.442115	51.006196
3449.313104	331402.885361	51.011201
3448.520191	331224.316187	51.016205
3447.727068	331022.146312	51.021210
3447.061311	330837.955159	51.026215
3446.394447	330641.594355	51.031220
3445.595305	330463.049781	51.036225
3444.920847	330267.503876	51.041229
3444.260263	330066.685226	51.046234
3443.561044	329887.257864	51.051239
3442.803210	329707.864801	51.056244
3442.060864	329511.309288	51.061249
3441.476964	329325.930336	51.066253
3441.011163	329151.148844	51.071258
3440.537985	328964.249397	51.076263
3439.609219	328775.639361	51.081268
3439.096096	328577.492161	51.086273
3438.339504	328396.262719	51.091277
3437.474211	328207.844932	51.096282
3436.841237	328007.449304	51.101287
3436.046512	327827.981290	51.106292
3435.425077	327647.263387	51.111297
3434.638952	327459.187712	51.116301
3434.041762	327292.748212	51.121306
3433.349533	327094.014519	51.126311
3432.964635	326906.892490	51.131316
3431.952871	326738.353262	51.136321
3431.396528	326543.415740	51.141325
3430.652786	326356.018175	51.146330
3429.906600	326178.626497	51.151335
3429.339730	326002.173573	51.156340
3428.799942	325814.284212	51.161345
3428.174282	325612.328297	51.166349
3427.528173	325434.435415	51.171354
3426.654835	325255.814256	51.176359
3425.935427	325082.591507	51.181364
3425.144310	324902.810848	51.186369
3424.455772	324705.496510	51.191373
3423.520385	324536.558731	51.196378
3423.291941	324346.019774	51.201383
3422.866389	324168.929509	51.206388
3421.896260	323985.916167	51.211393
3421.555097	323805.629159	51.216397
3420.770255	323631.497145	51.221402
3420.354469	323429.553668	51.226407
3419.595092	323252.106890	51.231412
3418.441591	323070.597326	51.236417
3417.888119	322884.638599	51.241421
3417.224102	322705.011392	51.246426
3416.677384	322517.013890	51.251431
3415.888658	322342.523417	51.256436
3415.365857	322157.958668	51.261441
3414.822764	321975.815598	51.266445
3413.505558	321810.115521	51.271450
3413.153634	321607.775779	51.276455
3412.733941	321442.646023	51.281460
3411.700454	321251.259977	51.286465
3411.196610	321084.589690	51.291469
3410.550326	320899.558070	51.296474
3410.166418	320711.072669	51.301479
3409.456117	320533.027016	51.306484
3408.736154	320349.482722	51.311489
3408.139767	320168.821206	51.316493
3407.556633	319990.117830	51.321498
3406.574834	319805.468047	51.326503
3406.031942	319631.900994	51.331508
3405.232829	319443.045777	51.336513
3404.722935	319256.003201	51.341517
3404.084739	319082.068255	51.346522
3403.540023	318896.176277	51.351527
3402.810330	318712.324727	51.356532
3401.752075	318540.976002	51.361537
3401.606739	318344.834735	51.366541
3400.442119	318174.775304	51.371546
3400.240278	317985.568097	51.376551
3399.534613	317810.037336	51.381556
3398.943103	317628.988225	51.386561
3398.426361	317439.778819	51.391565
3397.633823	317250.485343	51.396570
3397.125377	317066.341032	51.401575
3396.151359	316889.552436	51.406580
3395.509642	316686.407581	51.411585
3394.837513	316508.577504	51.416589
3393.986419	316326.217496	51.421594
3393.289732	316142.177627	51.426599
3392.584829	315968.705990	51.431604
3391.894285	315782.296407	51.436609
3391.366931	315606.071494	51.441613
3390.746636	315422.756676	51.446618
3389.711487	315229.780084	51.451623
3389.452472	315063.671732	51.456628
3388.304219	314885.990495	51.461633
3388.196892	314698.391781	51.466637
3387.244716	314528.903673	51.471642
3386.333905	314348.994098	51.476647
3385.631981	314165.409868	51.481652
3385.291224	313989.738369	51.486657
3384.784115	313813.099798	51.491661
3383.620568	313629.078364	51.496666
3383.333078	313453.270239	51.501671
3382.578312	313281.177068	51.506676
3381.695700	313102.024850	51.511681
3381.364560	312915.578805	51.516685
3380.624608	312753.158788	51.521690
3379.901603	312569.473316	51.526695
3378.984414	312394.908950	51.531700
3378.393321	312214.028547	51.536705
3377.927660	312041.352965	51.541709
3377.252165	311853.049767	51.546714
3376.779738	311674.899870	51.551719
3375.791888	311504.852475	51.556724
3375.300080	311332.791086	51.561729
3374.729519	311137.823897	51.566733
3373.752332	310981.855873	51.571738
3373.058209	310788.460965	51.576743
3372.486861	310622.395254	51.581748
3371.701164	310434.972945	51.586753
3371.430905	310260.175676	51.591757
3370.342790	310081.636856	51.596762
3370.086476	309904.595964	51.601767
3369.105046	309730.572462	51.606772
3368.269252	309557.416943	51.611777
3367.789257	309379.468449	51.616781
3367.063954	309205.683794	51.621786
3366.252727	309026.794036	51.626791
3365.593711	308853.278509	51.631796
3364.810796	308678.076177	51.636801
3364.499120	308510.056599	51.641805
3363.930448	308345.668005	51.646810
3363.072065	308161.487720	51.651815
3362.522622	307988.743071	51.656820
3361.647159	307814.725557	51.661825
3361.579762	307635.919882	51.666829
3360.417918	307471.063721	51.671834
3360.040356	307295.286051	51.676839
3359.344400	307116.757312	51.681844
3358.333536	306940.901057	51.686849
3358.049773	306758.308583	51.691853
3356.986063	306576.959679	51.696858
3356.757349	306402.837978	51.701863
3356.328732	306237.736968	51.706868
3354.978557	306048.716612	51.711873
3354.219337	305874.219741	51.716877
3354.024128	305690.873293	51.721882
3353.473169	305529.305007	51.726887
3352.733393	305336.061693	51.731892
3351.920225	305157.752590	51.736897
3351.235399	304986.349627	51.741901
3350.398132	304834.502766	51.746906
3349.913638	304637.067190	51.751911
3349.258032	304461.049659	51.756916
3348.003991	304296.382443	51.761921
3347.707063	304125.604658	51.766925
3346.799186	303956.196587	51.771930
3346.012793	303782.057910	51.776935
3345.724315	303608.553323	51.781940
3345.038480	303433.074096	51.786945
3344.451409	303272.807703	51.791949
3343.461400	303093.861870	51.796954
3343.170259	302924.405993	51.801959
3342.513472	302754.014576	51.806964
3341.598216	302588.298676	51.811969
3341.510023	302407.070241	51.816973
3340.391764	302238.763053	51.821978
3339.834668	302065.833944	51.826983
3338.891219	301896.938478	51.831988
3338.398136	301717.632299	51.836993
3337.950973	301542.367791	51.841997
3336.848146	301378.411963	51.847002
3336.385088	301205.849023	51.852007
3335.864645	301034.670156	51.857012
3335.121184	300867.320871	51.862017
3334.580855	300686.645815	51.867021
3333.895120	300507.343276	51.872026
3333.190477	300337.822658	51.877031
3332.601747	300160.032386	51.882036
3331.842257	299984.917451	51.887041
3331.610510	299810.457394	51.892045
3330.676209	299646.676904	51.897050
3330.012029	299458.660256	51.902055
3329.479236	299284.221805	51.907060
3328.475883	299114.365200	51.912065
3327.735723	298930.765725	51.917069
3327.074210	298777.739138	51.922074
3326.376064	298592.146259	51.927079
3325.745646	298431.652701	51.932084
3325.091207	298252.826713	51.937089
3324.663862	298082.852546	51.942093
3323.813540	297915.848338	51.947098
3322.772568	297735.122030	51.952103
3322.672459	297556.895289	51.957108
3321.792756	297397.942792	51.962113
3321.107328	297225.843966	51.967117
3320.528397	297048.405547	51.972122
3320.174299	296878.826163	51.977127
3319.340221	296716.198634	51.982132
3318.082175	296541.719460	51.987137
3318.027256	296362.975111	51.992141
3316.739831	296198.432424	51.997146
3316.496565	296026.389929	52.002151
3315.954230	295863.995687	52.007156
3315.370854	295697.736802	52.012161
3314.511854	295517.565379	52.017165
3313.657259	295343.938164	52.022170
3313.084994	295170.928293	52.027175
3312.655673	295005.281161	52.032180
3311.625193	294829.567557	52.037185
3311.169287	294649.484430	52.042189
3310.244243	294493.312722	52.047194
3309.761067	294330.653253	52.052199
3309.233594	294160.258607	52.057204
3308.675417	293983.552787	52.062209
3308.114223	293812.679327	52.067213
3307.265845	293640.399520	52.072218
3306.420263	293476.472443	52.077223
3305.827046	293295.009222	52.082228
3305.248069	293136.005877	52.087233
3304.718164	292961.153910	52.092237
3303.894806	292788.742171	52.097242
3303.553892	292616.890685	52.102247
3302.773239	292450.864284	52.107252
3301.798072	292268.212779	52.112257
3301.363751	292090.085215	52.117261
3300.433016	291930.703760	52.122266
3300.122999	291751.053705	52.127271
3299.297226	291575.432577	52.132276
3298.436189	291407.966541	52.137281
3298.045306	291236.376678	52.142285
3297.320034	291067.004343	52.147290
3296.665258	290900.269385	52.152295
3295.891750	290727.262587	52.157300
3294.996659	290549.792596	52.162305
3294.686254	290395.914972	52.167309
3293.787873	290224.073653	52.172314
3293.154269	290045.415929	52.177319
3292.420268	289885.543705	52.182324
3291.746636	289717.232012	52.187329
3291.215740	289543.982361	52.192333
3290.535020	289378.243838	52.197338
3289.495658	289204.335849	52.202343
3289.246291	289036.618820	52.207348
3288.128498	288879.047923	52.212353
3287.817790	288703.649127	52.217357
3287.147318	288544.428296	52.222362
3286.240248	288370.116890	52.227367
3285.679089	288213.832877	52.232372
3285.177966	288046.460753	52.237377
3284.898872	287868.458769	52.242381
3283.994903	287705.199592	52.247386
3283.403802	287536.440707	52.252391
3282.621623	287369.163637	52.257396
3281.701498	287197.706091	52.262401
3280.976682	287036.608503	52.267405
3280.261805	286860.457687	52.272410
3279.573056	286700.067347	52.277415
3279.164360	286529.165283	52.282420
3278.378859	286375.768342	52.287425
3277.912906	286196.037778	52.292429
3277.174235	286032.700757	52.297434
3276.529484	285881.140522	52.302439
3275.990116	285699.460301	52.307444
3275.221479	285541.297835	52.312449
3274.568082	285353.803307	52.317453
3273.686151	285201.923783	52.322458
3272.851634	285031.037494	52.327463
3272.475162	284867.948331	52.332468
3271.348965	284705.741746	52.337473
3270.898227	284541.365336	52.342477
3270.247281	284382.266975	52.347482
3269.699355	284221.776983	52.352487
3269.211813	284059.723825	52.357492
3268.420119	283886.258047	52.362497
3267.864134	283721.643318	52.367501
3267.033673	283563.540873	52.372506
3266.191434	283388.707635	52.377511
3266.007911	283221.308729	52.382516
3265.117299	283066.959475	52.387521
3264.826728	282893.235814	52.392525
3264.102634	282726.176949	52.397530
3263.208920	282557.056470	52.402535
3262.529917	282393.377651	52.407540
3261.683136	282229.878138	52.412545
3261.356195	282060.973481	52.417549
3260.620424	281905.351481	52.422554
3259.501975	281727.174154	52.427559
3259.213482	281565.419869	52.432564
3258.354195	281419.648050	52.437569
3257.700619	281240.123642	52.442573
3257.074057	281088.839258	52.447578
3256.435134	280912.903481	52.452583
3255.551771	280752.083570	52.457588
3255.316574	280596.993336	52.462593
3254.632533	280415.869049	52.467597
3253.736677	280265.824117	52.472602
3253.079749	280091.419110	52.477607
3252.763759	279926.714506	52.482612
3251.280203	279778.723524	52.487617
3250.809900	279613.941404	52.492621
3250.267405	279451.029866	52.497626
3249.641946	279291.849807	52.502631
3248.735684	279128.078905	52.507636
3247.907669	278975.909172	52.512641
3247.797163	278812.368899	52.517645
3246.902734	278662.756469	52.522650
3246.382048	278492.608333	52.527655
3245.697385	278325.083889	52.532660
3244.883844	278173.650357	52.537665
3244.694723	278008.517917	52.542669
3243.758040	277850.660336	52.547674
3243.302511	277689.950572	52.552679
3242.683741	277517.551163	52.557684
3241.703845	277362.323621	52.562689
3241.312402	277193.173645	52.567693
3240.481847	277035.502961	52.572698
3239.848813	276869.651136	52.577703
3238.990416	276703.885891	52.582708
3238.054988	276542.309641	52.587713
3237.646054	276390.251677	52.592717
3237.262967	276236.126679	52.597722
3236.517042	276072.864989	52.602727
3235.659536	275912.702623	52.607732
3234.946298	275750.225276	52.612737
3234.558249	275589.173650	52.617741
3234.097038	275437.760650	52.622746
3233.352432	275268.131646	52.627751
3232.501949	275110.565944	52.632756
3231.762523	274940.019264	52.637761
3230.974879	274784.073605	52.642765
3230.356388	274618.270391	52.647770
3229.863244	274453.033126	52.652775
3229.137212	274314.396241	52.657780
3228.403670	274149.426238	52.662785
3227.657032	273981.045552	52.667789
3227.154833	273828.289262	52.672794
3226.681508	273660.705816	52.677799
3226.240235	273504.909171	52.682804
3225.112068	273333.150662	52.687809
3224.506533	273174.171016	52.692813
3224.003053	273019.606736	52.697818
3223.255226	272848.042788	52.702823
3222.631886	272687.767119	52.707828
3221.899841	272527.508667	52.712833
3221.185118	272364.267695	52.717837
3220.642233	272200.286444	52.722842
3219.846075	272047.296677	52.727847
3219.143391	271879.036599	52.732852
3218.402105	271732.812775	52.737857
3217.829419	271563.717193	52.742861
3216.914114	271415.279730	52.747866
3216.514272	271243.915642	52.752871
3215.876002	271089.347468	52.757876
3214.876329	270936.135381	52.762881
3214.469661	270768.210686	52.767885
3213.778395	270609.728859	52.772890
3213.255034	270458.962865	52.777895
3212.438566	270295.967548	52.782900
3211.730781	270143.677225	52.787905
3211.415776	269974.541184	52.792909
3210.483071	269834.944252	52.797914
3209.638748	269657.614834	52.802919
3209.050529	269509.609868	52.807924
3208.308230	269345.533363	52.812929
3207.889354	269193.630498	52.817933
3207.352489	269031.941056	52.822938
3206.262247	268870.874039	52.827943
3205.674419	268716.018235	52.832948
3205.128243	268557.768604	52.837953
3204.626556	268403.765173	52.842957
3204.003052	268243.897896	52.847962
3202.936970	268084.610050	52.852967
3202.185382	267918.956377	52.857972
3201.793086	267766.412972	52.862977
3201.373665	267615.376528	52.867981
3200.779879	267455.759465	52.872986
3199.753791	267291.855791	52.877991
3199.125903	267137.414267	52.882996
3198.191423	266983.683472	52.888001
3197.827196	266833.886473	52.893005
3197.114671	266671.945384	52.898010
3196.410331	266513.950619	52.903015
3195.755139	266364.454490	52.908020
3194.900145	266213.512871	52.913025
3194.701585	266049.656985	52.918029
3194.020672	265897.669209	52.923034
3193.297278	265732.750417	52.928039
3192.748078	265568.491768	52.933044
3191.883216	265411.796210	52.938049
3191.392129	265255.652810	52.943053
3190.648175	265098.658096	52.948058
3189.610653	264927.702470	52.953063
3189.428897	264775.483334	52.958068
3188.363045	264629.873017	52.963073
3187.813440	264475.063528	52.968077
3187.251272	264305.357311	52.973082
3186.343351	264153.635344	52.978087
3185.733818	264007.316377	52.983092
3184.902854	263856.524675	52.988097
3184.683190	263689.489633	52.993101
3183.818291	263532.310984	52.998106
3183.513601	263387.905078	53.003111
3182.994142	263228.303397	53.008116
3181.747659	263084.988947	53.013121
3181.038096	262912.428863	53.018125
3180.358776	262756.265404	53.023130
3179.586828	262602.205043	53.028135
3179.171121	262453.844129	53.033140
3178.231285	262312.238790	53.038145
3177.854121	262146.961272	53.043149
3176.978243	261997.068914	53.048154
3176.462598	261837.390929	53.053159
3176.123603	261687.184567	53.058164
3174.731054	261540.328453	53.063169
3174.484522	261376.966244	53.068173
3173.589709	261238.206684	53.073178
3172.717253	261083.806458	53.078183
3172.352604	260933.528145	53.083188
3171.471038	260778.492836	53.088193
3170.962864	260628.899557	53.093197
3170.448780	260483.866012	53.098202
3169.938117	260331.140765	53.103207
3169.439577	260171.359144	53.108212
3168.536069	260023.840699	53.113217
3167.979112	259861.470810	53.118221
3167.256894	259717.642126	53.123226
3166.442385	259553.428578	53.128231
3165.921322	259412.089529	53.133236
3165.049270	259252.138368	53.138241
3164.983632	259103.138096	53.143245
3163.802523	258952.786361	53.148250
3162.983096	258796.061544	53.153255
3162.571133	258638.355525	53.158260
3161.532878	258494.017268	53.163265
3161.128903	258345.580343	53.168269
3160.530336	258182.224905	53.173274
3159.656497	258031.952464	53.178279
3159.213690	257880.160276	53.183284
3158.403672	257734.360196	53.188289
3157.843482	257581.364343	53.193293
3157.166777	257430.246147	53.198298
3156.564505	257275.678181	53.203303
3156.007665	257125.789124	53.208308
3155.204903	256972.169917	53.213313
3154.593580	256821.907678	53.218317
3153.714069	256672.757604	53.223322
3152.942746	256528.072753	53.228327
3152.317474	256367.549728	53.233332
3151.373499	256218.715777	53.238337
3151.155861	256066.328927	53.243341
3150.305640	255926.241070	53.248346
3149.615495	255780.474264	53.253351
3149.400120	255625.922667	53.258356
3148.311532	255489.540096	53.263361
3147.811264	255326.247642	53.268365
3147.275464	255176.585842	53.273370
3146.713245	255024.865501	53.278375
3145.784887	254866.887380	53.283380
3145.109121	254730.159865	53.288385
3144.816755	254570.400520	53.293389
3143.928574	254430.727184	53.298394
3142.912109	254282.517342	53.303399
3142.574231	254128.903107	53.308404
3141.789750	253972.227230	53.313409
3140.811306	253833.027020	53.318413
3140.362434	253685.517304	53.323418
3139.796130	253526.846323	53.328423
3139.339793	253383.743799	53.333428
3138.356802	253243.296873	53.338433
3138.168921	253073.513791	53.343437
3137.212103	252943.682620	53.348442
3136.370934	252786.889386	53.353447
3135.815044	252634.456895	53.358452
3135.153725	252489.120972	53.363457
3134.557183	252344.895452	53.368461
3133.677556	252195.519641	53.373466
3133.065344	252063.113381	53.378471
3132.100172	251903.284553	53.383476
3131.619038	251754.457263	53.388481
3130.880139	251614.889804	53.393485
3130.659814	251462.252438	53.398490
3129.679102	251325.372008	53.403495
3129.375905	251180.209715	53.408500
3128.707730	251028.356674	53.413505
3128.296140	250871.548134	53.418509
3127.289029	250709.995350	53.423514
3126.509294	250570.155094	53.428519
3126.264366	250419.636292	53.433524
3125.228158	250268.275121	53.438529
3124.712686	250127.553036	53.443533
3123.919802	249964.948438	53.448538
3123.181825	249825.942608	53.453543
3122.526947	249674.725386	53.458548
3122.041737	249526.486482	53.463553
3121.254619	249377.786169	53.468557
3120.426958	249238.387590	53.473562
3119.674453	249090.649791	53.478567
3119.261607	248940.821088	53.483572
3118.480457	248801.950334	53.488577
3117.797654	248649.745350	53.493581
3117.162287	248501.047336	53.498586
3116.352438	248359.201993	53.503591
3116.128125	248201.984483	53.508596
3115.294819	248058.003988	53.513601
3114.270839	247916.524010	53.518605
3113.560626	247776.369679	53.523610
3112.752335	247635.339693	53.528615
3112.295969	247472.353440	53.533620
3111.274002	247344.192385	53.538625
3110.745931	247208.211653	53.543629
3110.266810	247059.617696	53.548634
3109.548591	246932.885960	53.553639
3108.901788	246795.931240	53.558644
3108.614080	246651.891265	53.563649
3107.970477	246506.328880	53.568653
3106.724271	246370.666320	53.573658
3106.317182	246226.009029	53.578663
3106.385798	246076.565455	53.583668
3105.306908	245936.751398	53.588673
3104.337980	245787.981643	53.593677
3103.808222	245642.045629	53.598682
3103.145649	245491.979899	53.603687
3102.525878	245351.177024	53.608692
3101.894763	245198.050775	53.613697
3101.421852	245058.319982	53.618701
3100.222616	244921.301757	53.623706
3099.658290	244782.553407	53.628711
3099.199031	244630.317368	53.633716
3098.487355	244489.377153	53.638721
3098.037119	244342.946127	53.643725
3097.572274	244204.208108	53.648730
3096.393489	244061.381447	53.653735
3096.077886	243912.561324	53.658740
3095.107743	243759.464936	53.663745
3094.914488	243620.582701	53.668749
3093.967487	243482.049089	53.673754
3092.953417	243335.250064	53.678759
3092.693552	243197.448369	53.683764
3092.163462	243048.332151	53.688769
3091.438140	242899.247007	53.693773
3090.777160	242755.041148	53.698778
3089.817177	242597.921082	53.703783
3089.484092	242463.060260	53.708788
3088.510997	242330.847369	53.713793
3088.201244	242175.713062	53.718797
3087.360218	242026.774607	53.723802
3086.247641	241888.650948	53.728807
3085.896702	241741.927119	53.733812
3085.272832	241604.337598	53.738817
3084.623638	241456.770049	53.743821
3084.098473	241315.320057	53.748826
3083.339492	241172.099242	53.753831
3082.808660	241025.430225	53.758836
3081.649602	240885.583483	53.763841
3081.543605	240742.005199	53.768845
3080.570934	240599.200869	53.773850
3079.836575	240450.731329	53.778855
3079.435180	240308.906454	53.783860
3078.371446	240174.749532	53.788865
3077.716449	240025.987867	53.793869
3076.989250	239898.093195	53.798874
3076.490140	239763.057997	53.803879
3075.978814	239615.139918	53.808884
3075.252396	239473.520302	53.813889
3074.581073	239326.289994	53.818893
3073.791521	239186.157660	53.823898
3073.092949	239053.854090	53.828903
3072.545885	238901.715538	53.833908
3072.061962	238761.280724	53.838913
3071.533656	238619.656296	53.843917
3070.845606	238482.106127	53.848922
3069.996038	238328.717569	53.853927
3069.322644	238184.672112	53.858932
3068.485543	238070.802152	53.863937
3068.089288	237916.858610	53.868941
3067.403903	237772.790132	53.873946
3066.641911	237636.806033	53.878951
3066.037169	237494.252999	53.883956
3065.117217	237357.148379	53.888961
3064.582591	237217.614815	53.893965
3063.971490	237079.061162	53.898970
3063.408356	236928.735843	53.903975
3062.745466	236787.669856	53.908980
3061.847326	236662.759804	53.913985
3061.647713	236502.854140	53.918989
3060.839329	236361.251554	53.923994
3060.168099	236212.752286	53.928999
3059.560538	236073.893837	53.934004
3058.674342	235935.945433	53.939009
3058.166866	235783.575875	53.944013
3057.136964	235636.738403	53.949018
3056.392899	235505.083015	53.954023
3055.852246	235356.538855	53.959028
3055.056379	235226.165195	53.964033
3054.571222	235096.506426	53.969037
3054.323821	234945.624757	53.974042
3053.535390	234815.301379	53.979047
3052.839740	234653.643760	53.984052
3051.967580	234519.616394	53.989057
3051.461109	234380.209538	53.994061
3050.965075	234248.847560	53.999066
3050.149245	234095.408985	54.004071
3049.586851	233960.391216	54.009076
3048.572155	233818.875774	54.014081
3048.021531	233675.453755	54.019085
3047.573348	233529.367591	54.024090
3046.563620	233401.067214	54.029095
3046.256121	233254.017072	54.034100
3045.323591	233116.741941	54.039105
3044.500526	232977.463586	54.044109
3043.817625	232843.026627	54.049114
3043.122044	232710.858042	54.054119
3042.746173	232568.861383	54.059124
3041.888511	232428.672650	54.064129
3041.293986	232282.764324	54.069133
3040.788189	232158.103391	54.074138
3040.045359	232018.457268	54.079143
3039.182707	231885.857957	54.084148
3038.599012	231746.161591	54.089153
3038.188654	231605.597739	54.094157
3037.684051	231465.965661	54.099162
3036.270916	231331.340898	54.104167
3036.043716	231181.938741	54.109172
3035.206971	231064.741176	54.114177
3034.786698	230924.154469	54.119181
3034.065322	230784.073956	54.124186
3033.312605	230648.174406	54.129191
3032.687028	230497.283234	54.134196
3031.950500	230377.040705	54.139201
3031.422999	230232.601809	54.144205
3030.545034	230097.563157	54.149210
3030.035243	229967.100503	54.154215
3029.506016	229820.269123	54.159220
3028.850380	229691.103050	54.164225
3028.209240	229541.234422	54.169229
3027.492464	229404.287133	54.174234
3026.624937	229265.403365	54.179239
3026.408954	229109.713823	54.184244
3025.787750	228981.128956	54.189249
3024.787855	228830.045241	54.194253
3024.074385	228696.281231	54.199258
3023.430932	228568.158803	54.204263
3022.877417	228416.750534	54.209268
3022.199828	228281.988486	54.214273
3021.474635	228145.299117	54.219277
3020.833158	227998.514018	54.224282
3020.182953	227873.118055	54.229287
3019.766034	227730.677216	54.234292
3019.014545	227589.919092	54.239297
3018.350842	227448.587159	54.244301
3017.790568	227304.947587	54.249306
3016.768767	227173.348033	54.254311
3016.271849	227033.518060	54.259316
3015.481546	226891.977949	54.264321
3014.765015	226746.619983	54.269325
3014.270690	226610.405764	54.274330
3013.434211	226486.759958	54.279335
3012.848909	226336.518903	54.284340
3012.012150	226208.290603	54.289345
3011.462542	226071.131239	54.294349
3010.602984	225934.784987	54.299354
3009.910959	225789.997686	54.304359
3009.524791	225651.858374	54.309364
3008.546719	225521.260215	54.314369
3007.926075	225395.735989	54.319373
3007.426744	225258.366343	54.324378
3006.581484	225126.131053	54.329383
3006.102151	225003.029272	54.334388
3005.349278	224863.243499	54.339393
3004.824509	224718.622585	54.344397
3004.149801	224589.696483	54.349402
3003.071816	224468.090602	54.354407
3002.568371	224326.318571	54.359412
3001.946579	224197.562948	54.364417
3001.452332	224063.198844	54.369421
3000.719595	223930.604005	54.374426
3000.449339	223798.878203	54.379431
2999.827676	223674.337050	54.384436
2998.663850	223535.382462	54.389441
2998.335927	223390.007200	54.394445
2997.662241	223258.333435	54.399450
2996.798897	223119.090154	54.404455
2996.363494	222985.966109	54.409460
2995.586274	222849.281118	54.414465
2994.880307	222705.672780	54.419469
2994.241248	222576.158766	54.424474
2993.648121	222447.337838	54.429479
2993.196326	222310.831423	54.434484
2992.273795	222174.718012	54.439489
2991.666240	222028.867652	54.444493
2991.182122	221901.188794	54.449498
2990.007055	221763.703095	54.454503
2989.797611	221617.064913	54.459508
2989.010267	221492.018866	54.464513
2988.461596	221344.823888	54.469517
2987.768131	221211.832891	54.474522
2986.886897	221077.840758	54.479527
2986.327657	220948.558747	54.484532
2985.438271	220804.346563	54.489537
2984.973859	220664.420876	54.494541
2984.542478	220534.686538	54.499546
2983.455904	220412.553800	54.504551
2982.996759	220264.659389	54.509556
2982.532114	220132.003253	54.514561
2981.637905	219994.514542	54.519565
2981.074661	219857.533788	54.524570
2979.988352	219728.770143	54.529575
2979.720609	219590.813867	54.534580
2978.894936	219466.846568	54.539585
2978.265664	219330.793764	54.544589
2977.654539	219189.837581	54.549594
2976.946999	219060.073196	54.554599
2976.449463	218930.861344	54.559604
2976.043196	218793.870474	54.564609
2975.342423	218654.495218	54.569613
2974.524420	218517.697346	54.574618
2973.728789	218384.027555	54.579623
2973.108971	218233.693272	54.584628
2971.739114	218108.019663	54.589633
2971.513634	217972.567422	54.594637
2970.820374	217839.417069	54.599642
2970.059694	217724.352804	54.604647
2969.519611	217583.108506	54.609652
2968.936831	217451.978030	54.614657
2968.001033	217326.211642	54.619661
2967.619997	217195.584322	54.624666
2966.789923	217068.999740	54.629671
2966.505909	216935.048041	54.634676
2965.607823	216809.887598	54.639681
2964.981884	216672.031872	54.644685
2964.448582	216540.627971	54.649690
2963.589978	216404.604367	54.654695
2963.109832	216271.092321	54.659700
2962.449194	216141.287702	54.664705
2961.487216	216011.976537	54.669709
2960.467650	215867.043950	54.674714
2959.772090	215756.924083	54.679719
2959.572593	215620.415833	54.684724
2958.823771	215511.959513	54.689729
2958.404948	215379.037744	54.694733
2957.758324	215251.880139	54.699738
2956.754900	215121.431661	54.704743
2956.607254	214987.296707	54.709748
2955.746077	214853.376809	54.714753
2955.274548	214720.031913	54.719757
2954.487061	214586.139068	54.724762
2953.509065	214446.688891	54.729767
2952.994924	214318.328339	54.734772
2952.256618	214176.435122	54.739777
2951.669768	214057.250984	54.744781
2951.125222	213929.176021	54.749786
2950.378243	213801.069712	54.754791
2949.730042	213661.314409	54.759796
2949.176662	213545.384322	54.764801
2948.669727	213402.997920	54.769805
2948.057071	213270.874728	54.774810
2947.073847	213145.072711	54.779815
2946.852609	213002.654676	54.784820
2945.764652	212882.495569	54.789825
2944.917179	212741.730074	54.794829
2944.612390	212607.357533	54.799834
2943.533076	212477.269948	54.804839
2943.064153	212347.582381	54.809844
2942.393182	212216.043325	54.814849
2941.900373	212074.255809	54.819853
2941.125146	211951.401516	54.824858
2940.192029	211825.034107	54.829863
2939.831132	211686.624906	54.834868
2938.826517	211553.816335	54.839873
2938.500931	211427.773546	54.844877
2937.960740	211306.996096	54.849882
2936.984912	211181.400392	54.854887
2936.418779	211040.352264	54.859892
2935.608279	210931.480558	54.864897
2934.778818	210787.369128	54.869901
2934.359335	210664.995563	54.874906
2933.567809	210540.568355	54.879911
2933.255925	210410.096217	54.884916
2932.742387	210279.707187	54.889921
2931.796167	210150.710596	54.894925
2931.228718	210021.730669	54.899930
2930.772063	209892.351643	54.904935
2929.929158	209746.081070	54.909940
2929.115901	209627.653756	54.914945
2928.495828	209487.483136	54.919949
2927.523710	209367.045089	54.924954
2927.158768	209252.391183	54.929959
2926.367109	209105.032192	54.934964
2925.337910	208988.943941	54.939969
2924.910551	208864.131533	54.944973
2924.220256	208732.551934	54.949978
2923.489115	208612.064492	54.954983
2923.004820	208482.590990	54.959988
2922.141916	208369.213936	54.964993
2921.877607	208235.073443	54.969997
2921.277210	208105.288222	54.975002
2920.574306	207982.812130	54.980007
2919.972339	207847.262342	54.985012
2919.426323	207730.425464	54.990017
2918.340378	207583.753109	54.995021
2917.767713	207459.641132	55.000026
2917.005208	207336.564899	55.005031
2916.531883	207203.681584	55.010036
2915.701739	207095.927044	55.015041
2915.015736	206964.197904	55.020045
2914.574804	206836.808286	55.025050
2913.759217	206710.152783	55.030055
2913.076116	206572.162460	55.035060
2912.461380	206461.664162	55.040065
2911.911389	206327.700446	55.045069
2911.232191	206200.744453	55.050074
2910.329196	206084.272772	55.055079
2909.914215	205956.473692	55.060084
2909.222825	205826.058790	55.065089
2908.666641	205690.213969	55.070093
2907.990852	205559.377215	55.075098
2906.918428	205444.422645	55.080103
2906.611543	205314.024368	55.085108
2905.592317	205189.975149	55.090113
2905.160534	205055.677471	55.095117
2904.488108	204940.469671	55.100122
2903.561396	204818.621000	55.105127
2903.337213	204688.974621	55.110132
2902.253439	204573.094556	55.115137
2901.428534	204449.397955	55.120141
2901.196196	204317.692040	55.125146
2900.620113	204207.039195	55.130151
2900.265840	204071.967966	55.135156
2899.498637	203942.383802	55.140161
2898.649649	203813.818252	55.145165
2897.938819	203694.775732	55.150170
2897.294482	203560.896997	55.155175
2896.717224	203433.243745	55.160180
2895.884815	203305.923879	55.165185
2895.399716	203177.849377	55.170189
2894.683461	203046.363019	55.175194
2893.716985	202930.951323	55.180199
2893.168424	202799.973480	55.185204
2892.439751	202682.933898	55.190209
2891.848332	202554.826748	55.195213
2890.955915	202431.323413	55.200218
2890.456280	202316.526263	55.205223
2890.165911	202181.869397	55.210228
2889.400559	202056.476080	55.215233
2889.017535	201933.045904	55.220237
2888.209802	201801.653318	55.225242
2887.242858	201676.369137	55.230247
2886.523122	201543.334345	55.235252
2885.902285	201409.686108	55.240257
2885.397843	201293.428395	55.245261
2884.704330	201170.838076	55.250266
2883.741881	201050.072192	55.255271
2883.184325	200925.272101	55.260276
2882.260650	200803.457130	55.265281
2881.473904	200685.476566	55.270285
2881.309522	200560.602327	55.275290
2880.771576	200439.337915	55.280295
2880.124494	200315.406000	55.285300
2879.252172	200190.428379	55.290305
2878.641862	200061.579237	55.295309
2878.278097	199934.103871	55.300314
2877.269582	199819.888819	55.305319
2876.787687	199674.541056	55.310324
2876.205315	199561.060766	55.315329
2875.635081	199437.971288	55.320333
2875.105620	199304.517371	55.325338
2874.305597	199178.512644	55.330343
2873.429395	199050.700590	55.335348
2872.736026	198930.507648	55.340353
2872.030103	198798.622671	55.345357
2871.547209	198681.781819	55.350362
2870.554225	198569.195784	55.355367
2869.888168	198428.334316	55.360372
2869.243858	198310.323700	55.365377
2868.414999	198186.692728	55.370381
2867.969188	198063.841230	55.375386
2867.254003	197948.540315	55.380391
2866.349752	197822.555321	55.385396
2865.943725	197695.231986	55.390401
2865.280450	197576.526160	55.395405
2864.551378	197467.870809	55.400410
2863.775991	197330.974254	55.405415
2863.495023	197215.415327	55.410420
2862.416415	197096.000161	55.415425
2861.937041	196975.141575	55.420429
2861.661130	196855.688926	55.425434
2860.719287	196738.454274	55.430439
2860.198642	196605.540242	55.435444
2859.152019	196484.721729	55.440449
2858.511353	196356.891678	55.445453
2858.019380	196236.342201	55.450458
2856.876308	196120.642300	55.455463
2856.343320	196005.202333	55.460468
2856.175549	195889.921106	55.465473
2855.484297	195763.538391	55.470477
2854.805076	195635.232722	55.475482
2853.984145	195520.424762	55.480487
2853.513109	195398.270694	55.485492
2852.732045	195276.980359	55.490497
2851.887804	195156.769146	55.495501
2851.419968	195034.793583	55.500506
2850.112944	194920.000338	55.505511
2849.929408	194801.670296	55.510516
2849.317951	194675.417619	55.515521
2848.442670	194553.380501	55.520525
2848.231675	194453.467221	55.525530
2847.378978	194328.564183	55.530535
2846.473272	194206.888995	55.535540
2845.951774	194085.395013	55.540545
2845.507710	193971.943247	55.545549
2844.968716	193839.357457	55.550554
2844.347204	193718.350987	55.555559
2843.742638	193598.627224	55.560564
2842.876334	193478.092710	55.565569
2842.242316	193355.994864	55.570573
2841.572339	193226.332447	55.575578
2840.434714	193119.532409	55.580583
2839.898504	192987.152031	55.585588
2839.455268	192872.481183	55.590593
2838.731752	192755.017642	55.595597
2838.247200	192630.874880	55.600602
2837.050088	192528.386083	55.605607
2836.882294	192390.630562	55.610612
2836.076912	192280.026324	55.615617
2835.335148	192148.876755	55.620621
2834.755185	192040.832926	55.625626
2833.998656	191917.651123	55.630631
2833.476923	191802.867976	55.635636
2833.075593	191678.014674	55.640641
2831.975209	191559.404981	55.645645
2831.355827	191442.169848	55.650650
2830.669088	191321.077831	55.655655
2829.946973	191203.452405	55.660660
2829.546683	191087.697485	55.665665
2828.785481	190973.526765	55.670669
2828.191196	190850.881796	55.675674
2827.288115	190740.487388	55.680679
2826.712186	190606.961980	55.685684
2825.874126	190502.728456	55.690689
2825.532970	190391.406150	55.695693
2825.168860	190275.380276	55.700698
2824.036894	190163.992894	55.705703
2823.528974	190037.748490	55.710708
2822.898626	189908.368563	55.715713
2822.360162	189792.689545	55.720717
2821.367577	189670.072516	55.725722
2820.343589	189562.460811	55.730727
2820.166344	189449.727975	55.735732
2819.745610	189337.428370	55.740737
2818.669236	189217.713818	55.745741
2818.368818	189087.940370	55.750746
2817.262785	188973.701831	55.755751
2816.785705	188849.656706	55.760756
2816.063687	188751.439114	55.765761
2815.315321	188629.854801	55.770765
2815.212380	188512.341531	55.775770
2814.010106	188395.447941	55.780775
2813.662515	188271.371117	55.785780
2813.095569	188153.792288	55.790785
2812.095351	188031.575136	55.795789
2811.764048	187904.761422	55.800794
2811.069248	187794.175531	55.805799
2810.558166	187677.823111	55.810804
2809.764981	187552.762833	55.815809
2809.238859	187430.383126	55.820813
2808.347486	187308.099756	55.825818
2807.551761	187193.803719	55.830823
2806.952568	187067.479996	55.835828
2806.331180	186964.136003	55.840833
2805.439721	186842.642645	55.845837
2804.893268	186713.499994	55.850842
2804.385580	186604.579335	55.855847
2803.961549	186489.844527	55.860852
2803.158731	186361.901156	55.865857
2802.353276	186251.120228	55.870861
2801.708211	186116.015650	55.875866
2801.255511	186004.632418	55.880871
2800.646907	185879.458418	55.885876
2799.661758	185761.506678	55.890881
2798.547077	185653.104240	55.895885
2798.456672	185523.523807	55.900890
2797.648783	185422.744438	55.905895
2797.116468	185298.552241	55.910900
2796.118016	185184.509615	55.915905
2795.582544	185065.737907	55.920909
2795.007385	184958.231242	55.925914
2794.021735	184829.201674	55.930919
2793.576615	184719.537794	55.935924
2793.211480	184588.934966	55.940929
2792.336651	184493.142314	55.945933
2792.049425	184367.934333	55.950938
2790.874036	184255.130614	55.955943
2790.465024	184137.766112	55.960948
2789.991458	184011.074825	55.965953
2789.435234	183884.943998	55.970957
2788.713065	183763.393954	55.975962
2787.765006	183647.032039	55.980967
2787.095199	183530.740848	55.985972
2786.398280	183414.810444	55.990977
2785.432401	183302.293991	55.995981
2784.984730	183187.774893	56.000986
2784.118981	183072.673545	56.005991
2783.515325	182953.294949	56.010996
2783.188352	182850.130041	56.016001
2782.798763	182728.441126	56.021005
2782.142459	182606.769351	56.026010
2781.166595	182484.372564	56.031015
2780.665157	182363.007676	56.036020
2779.855317	182245.940661	56.041025
2779.300520	182121.481062	56.046029
2778.607874	182001.025186	56.051034
2777.758596	181892.360937	56.056039
2777.236005	181778.010039	56.061044
2776.396365	181656.637083	56.066049
2775.914014	181533.948556	56.071053
2775.189326	181418.218649	56.076058
2774.203408	181311.765405	56.081063
2773.580191	181183.261541	56.086068
2772.985701	181079.519902	56.091073
2772.256576	180976.804739	56.096077
2771.825730	180852.532677	56.101082
2771.257843	180744.831643	56.106087
2770.663771	180616.045012	56.111092
2769.939805	180503.026843	56.116097
2769.441794	180383.435061	56.121101
2768.796232	180248.106848	56.126106
2767.906909	180153.865139	56.131111
2766.910031	180023.388730	56.136116
2766.510205	179913.538934	56.141121
2765.835178	179792.183335	56.146125
2765.169859	179678.051431	56.151130
2764.502538	179565.077656	56.156135
2763.796503	179451.258087	56.161140
2763.004336	179333.267663	56.166145
2762.579731	179233.421291	56.171149
2762.057626	179096.512664	56.176154
2760.981260	179000.725902	56.181159
2760.373515	178866.426399	56.186164
2759.936351	178760.566751	56.191169
2759.217203	178646.611514	56.196173
2758.545402	178526.696349	56.201178
2757.875794	178421.001570	56.206183
2757.522516	178300.807648	56.211188
2756.639069	178186.510821	56.216193
2755.831336	178068.373779	56.221197
2755.412631	177938.956987	56.226202
2754.638107	177843.175940	56.231207
2753.767122	177715.039817	56.236212
2752.984316	177622.427691	56.241217
2752.425152	177493.505143	56.246221
2752.022453	177380.571652	56.251226
2751.226655	177272.584884	56.256231
2750.768401	177145.491709	56.261236
2750.039376	177034.684064	56.266241
2749.343649	176913.518147	56.271245
2748.502637	176798.277213	56.276250
2747.994337	176702.558388	56.281255
2747.458287	176570.595223	56.286260
2746.582374	176465.663081	56.291265
2746.234478	176345.512128	56.296269
2745.615431	176231.585823	56.301274
2744.327511	176111.444547	56.306279
2744.146919	176000.870786	56.311284
2743.356377	175883.118835	56.316289
2742.475009	175773.343503	56.321293
2742.268664	175642.920936	56.326298
2741.530265	175545.142688	56.331303
2740.856182	175410.674125	56.336308
2740.272647	175296.846553	56.341313
2739.509864	175169.642401	56.346317
2738.970012	175060.412667	56.351322
2737.852799	174950.409830	56.356327
2737.724894	174823.907459	56.361332
2736.796645	174718.212290	56.366337
2736.239191	174594.335068	56.371341
2735.722211	174465.504408	56.376346
2734.743720	174367.690727	56.381351
2734.238939	174247.316463	56.386356
2733.525807	174127.611470	56.391361
2732.776272	174017.349451	56.396365
2732.274226	173889.713776	56.401370
2731.413154	173776.862879	56.406375
2730.877232	173656.724246	56.411380
2730.133626	173535.626870	56.416385
2729.551527	173430.350830	56.421389
2729.039514	173302.807633	56.426394
2728.370231	173199.377392	56.431399
2727.930850	173067.003374	56.436404
2726.806306	172953.229993	56.441409
2726.077560	172834.078221	56.446413
2725.586115	172717.979622	56.451418
2724.885535	172614.403251	56.456423
2724.291805	172481.076379	56.461428
2723.630708	172381.564010	56.466433
2722.812909	172260.227929	56.471437
2722.558587	172125.538584	56.476442
2721.447776	172017.959158	56.481447
2720.742040	171901.566252	56.486452
2720.195819	171790.845825	56.491457
2719.538102	171681.237067	56.496461
2719.164941	171557.543594	56.501466
2718.050875	171436.155254	56.506471
2718.042274	171325.567172	56.511476
2717.110013	171205.511497	56.516481
2716.388871	171096.219640	56.521485
2716.155645	170964.659372	56.526490
2714.937462	170850.779749	56.531495
2714.373250	170735.423420	56.536500
2713.601596	170610.015689	56.541505
2712.662450	170492.303242	56.546509
2712.136388	170381.151248	56.551514
2711.209404	170267.570569	56.556519
2711.075567	170150.748943	56.561524
2710.247286	170034.152131	56.566529
2709.748575	169931.669985	56.571533
2709.422804	169817.626603	56.576538
2708.418796	169693.670217	56.581543
2707.608450	169572.468507	56.586548
2706.786852	169465.193696	56.591553
2706.406087	169346.200930	56.596557
2705.954434	169218.152848	56.601562
2705.170031	169109.639632	56.606567
2704.662589	168982.224287	56.611572
2703.894839	168864.146330	56.616577
2703.174925	168751.236742	56.621581
2702.534993	168626.094380	56.626586
2701.536309	168514.819202	56.631591
2701.334967	168385.093854	56.636596
2700.117703	168285.069749	56.641601
2699.618457	168171.567410	56.646605
2699.215633	168049.721037	56.651610
2698.258883	167940.691666	56.656615
2697.659086	167809.251151	56.661620
2697.204014	167696.455341	56.666625
2696.316553	167586.398732	56.671629
2696.267579	167474.391227	56.676634
2695.456246	167354.811677	56.681639
2694.494205	167230.678657	56.686644
2693.452742	167122.962097	56.691649
2693.053850	167000.826026	56.696653
2692.794266	166872.348538	56.701658
2691.666472	166769.618543	56.706663
2691.305314	166643.535778	56.711668
2690.788047	166529.850511	56.716673
2689.814026	166425.177037	56.721677
2689.517857	166297.050645	56.726682
2688.389885	166187.748324	56.731687
2687.914791	166059.015318	56.736692
2687.375855	165953.142567	56.741697
2686.509884	165830.041656	56.746701
2686.386699	165706.531025	56.751706
2685.041649	165589.991657	56.756711
2684.719990	165472.959929	56.761716
2684.175276	165346.440176	56.766721
2683.406274	165236.092006	56.771725
2682.808729	165108.869384	56.776730
2681.841354	164992.971406	56.781735
2681.399357	164868.598594	56.786740
2680.780361	164755.112902	56.791745
2679.955427	164647.534527	56.796749
2679.649989	164514.088187	56.801754
2678.826653	164410.985925	56.806759
2678.165186	164281.741906	56.811764
2677.399131	164166.361388	56.816769
2676.487900	164039.955062	56.821773
2675.909943	163939.447222	56.826778
2675.585146	163814.067673	56.831783
2674.859951	163695.020331	56.836788
2674.328733	163571.912104	56.841793
2673.244635	163457.690393	56.846797
2672.870597	163321.169635	56.851802
2672.228140	163206.993177	56.856807
2671.678992	163087.907222	56.861812
2671.047507	162975.268208	56.866817
2670.101549	162860.238203	56.871821
2669.596801	162725.850990	56.876826
2669.036990	162612.299036	56.881831
2668.667192	162492.538201	56.886836
2667.843282	162366.632453	56.891841
2667.067045	162248.627814	56.896845
2666.587996	162120.392455	56.901850
2665.783621	162003.092360	56.906855
2665.313368	161881.569504	56.911860
2664.357978	161743.341434	56.916865
2663.817841	161615.041279	56.921869
2663.612378	161499.822035	56.926874
2662.348715	161378.019749	56.931879
2661.696251	161244.665888	56.936884
2660.957690	161126.595417	56.941889
2660.065573	161013.355461	56.946893
2659.598180	160869.383141	56.951898
2658.534972	160760.010636	56.956903
2658.202478	160647.001029	56.961908
2657.404031	160528.942037	56.966913
2656.703674	160413.741155	56.971917
2656.412941	160293.797188	56.976922
2655.757643	160177.305877	56.981927
2655.073185	160053.051685	56.986932
2654.191786	159938.033602	56.991937
2653.385283	159813.443618	56.996941
2652.949705	159689.532678	57.001946
2652.434325	159583.891009	57.006951
2651.839148	159452.073140	57.011956
2651.288335	159330.025138	57.016961
2650.610342	159205.404242	57.021965
2649.735015	159083.739055	57.026970
2649.093726	158968.609835	57.031975
2648.416622	158838.904904	57.036980
2648.013276	158720.636842	57.041985
2647.232339	158603.064651	57.046989
2646.736452	158474.184130	57.051994
2645.701457	158352.902755	57.056999
2645.062466	158229.944544	57.062004
2644.706018	158110.107464	57.067009
2643.978770	157986.947984	57.072013
2643.152569	157856.011797	57.077018
2642.387509	157748.851607	57.082023
2641.951129	157614.956108	57.087028
2641.368176	157494.114626	57.092033
2640.544377	157376.464407	57.097037
2640.043558	157244.461996	57.102042
2639.395928	157126.505048	57.107047
2638.604205	157001.579580	57.112052
2637.768443	156878.301423	57.117057
2637.162320	156758.178086	57.122061
2636.688524	156636.572306	57.127066
2635.868693	156516.712496	57.132071
2635.730344	156388.761959	57.137076
2634.736660	156264.481362	57.142081
2633.781433	156148.279934	57.147085
2633.214076	156020.767398	57.152090
2632.560382	155898.913090	57.157095
2631.785131	155782.264906	57.162100
2631.531037	155654.475296	57.167105
2630.869413	155527.754966	57.172109
2630.655865	155393.604049	57.177114
2629.588558	155282.063111	57.182119
2628.913880	155139.469468	57.187124
2628.163944	155015.790407	57.192129
2627.283760	154889.844368	57.197133
2627.146955	154753.319495	57.202138
2626.198036	154633.283417	57.207143
2625.171720	154517.264106	57.212148
2624.858537	154393.924892	57.217153
2624.047750	154265.491492	57.222157
2623.582222	154140.829953	57.227162
2622.720350	154022.231348	57.232167
2621.986653	153893.405827	57.237172
2621.857594	153762.680026	57.242177
2620.602325	153643.827322	57.247181
2620.400266	153509.199086	57.252186
2619.536545	153393.437555	57.257191
2619.003387	153262.396417	57.262196
2618.287725	153136.316514	57.267201
2617.261862	153007.197522	57.272205
2616.912919	152881.136746	57.277210
2616.188728	152767.999121	57.282215
2615.822396	152638.255925	57.287220
2615.510687	152512.101679	57.292225
2614.377557	152388.493073	57.297229
2613.698641	152247.450430	57.302234
2613.064018	152121.895393	57.307239
2612.325080	151991.718071	57.312244
2611.310733	151869.630549	57.317249
2610.804851	151749.255065	57.322253
2610.382810	151612.597624	57.327258
2609.676009	151493.818272	57.332263
2608.763633	151360.544228	57.337268
2608.305924	151244.153950	57.342273
2607.479468	151135.880692	57.347277
2607.006494	150948.152416	57.352282
2606.153171	150804.893947	57.357287
2605.908722	150702.007885	57.362292
2605.465750	150555.800344	57.367297
2604.644615	150425.731250	57.372301
2604.249416	150287.232184	57.377306
2603.190416	150154.698051	57.382311
2602.334071	150039.836857	57.387316
2602.015685	149907.593089	57.392321
2601.023718	149767.996104	57.397325
2600.396810	149650.253006	57.402330
2600.036709	149514.280870	57.407335
2599.262666	149377.358151	57.412340
2598.766035	149264.946460	57.417345
2598.011290	149122.569467	57.422349
2597.928884	149001.298248	57.427354
2596.801762	148878.845858	57.432359
2596.155830	148719.893362	57.437364
2595.495725	148599.312531	57.442369
2594.703101	148464.938459	57.447373
2593.986592	148328.481332	57.452378
2593.043039	148215.102008	57.457383
2592.457927	148069.131615	57.462388
2591.987112	147960.189929	57.467393
2591.147308	147811.630351	57.472397
2590.528120	147689.152873	57.477402
2589.936740	147556.453708	57.482407
2589.662704	147432.143317	57.487412
2588.726019	147297.148864	57.492417
2588.234178	147175.047156	57.497421
2587.296248	147042.582976	57.502426
2586.911759	146916.106261	57.507431
2586.050997	146759.319902	57.512436
2585.717809	146642.075109	57.517441
2584.472675	146510.932669	57.522445
2583.988345	146384.359533	57.527450
2583.427447	146242.434922	57.532455
2582.559741	146108.095450	57.537460
2582.065299	145995.606018	57.542465
2581.339309	145851.739592	57.547469
2580.744002	145718.807329	57.552474
2580.056697	145602.664579	57.557479
2579.539812	145472.275216	57.562484
2579.267467	145333.562193	57.567489
2578.278248	145183.208773	57.572493
2577.739154	145062.088550	57.577498
2576.985935	144920.111460	57.582503
2576.527633	144783.552519	57.587508
2575.941029	144673.128369	57.592513
2574.840707	144496.618478	57.597517
2574.517763	144379.545741	57.602522
2573.728115	144249.636777	57.607527
2572.733357	144100.865184	57.612532
2572.023281	143991.149223	57.617537
2571.161364	143850.668294	57.622541
2571.153143	143712.746622	57.627546
2570.046175	143584.529958	57.632551
2569.402350	143466.406019	57.637556
2569.122305	143312.505712	57.642561
2567.937848	143204.151131	57.647565
2567.623524	143028.389154	57.652570
2566.832876	142938.220080	57.657575
2566.081187	142807.167581	57.662580
2565.688426	142648.307438	57.667585
2564.771201	142529.150372	57.672589
2564.738187	142395.025113	57.677594
2563.969758	142248.704405	57.682599
2563.022848	142133.263883	57.687604
2562.351492	141979.356054	57.692609
2561.556419	141872.177013	57.697613
2561.401798	141705.279062	57.702618
2560.519156	141616.958178	57.707623
2559.590765	141445.355917	57.712628
2559.318857	141339.213992	57.717633
2558.371512	141185.087102	57.722637
2557.815122	141067.174605	57.727642
2557.322301	140912.367188	57.732647
2556.269021	140784.306278	57.737652
2556.000443	140654.368154	57.742657
2555.286397	140504.540451	57.747661
2554.458572	140395.148334	57.752666
2553.837938	140230.759167	57.757671
2553.421588	140120.845437	57.762676
2552.881779	139956.584724	57.767681
2551.292257	139849.310078	57.772685
2551.286930	139689.514684	57.777690
2550.682205	139551.706435	57.782695
2549.733879	139444.827136	57.787700
2549.384048	139293.562891	57.792705
2548.192491	139164.361940	57.797709
2547.559277	139025.340942	57.802714
2547.206654	138904.584123	57.807719
2546.649396	138758.678892	57.812724
2545.940407	138611.909079	57.817729
2545.252907	138508.256981	57.822733
2544.815316	138354.279870	57.827738
2544.067577	138221.213946	57.832743
2543.499324	138067.602062	57.837748
2542.913272	137952.844624	57.842753
2542.130279	137793.792488	57.847757
2541.372523	137655.293138	57.852762
2540.711977	137520.221945	57.857767
2540.016926	137389.285777	57.862772
2539.544807	137229.501384	57.867777
2538.642494	137115.572298	57.872781
2538.074312	136960.644931	57.877786
2537.498296	136832.601651	57.882791
2536.645826	136702.582789	57.887796
2535.925453	136561.275068	57.892801
2535.323934	136434.368234	57.897805
2535.174721	136273.115035	57.902810
2534.090973	136151.494472	57.907815
2533.533179	135990.244072	57.912820
2532.954087	135871.898503	57.917825
2532.354637	135730.626460	57.922829
2531.582531	135579.575263	57.927834
2530.732328	135456.192904	57.932839
2530.264768	135313.949218	57.937844
2529.299734	135157.595322	57.942849
2528.940392	135054.614842	57.947853
2528.655950	134870.042023	57.952858
2527.444265	134769.776419	57.957863
2527.002916	134602.849625	57.962868
2526.360388	134488.127479	57.967873
2525.404516	134352.330202	57.972877
2525.118717	134189.839935	57.977882
2524.491304	134079.118478	57.982887
2523.693825	133896.564061	57.987892
2523.112638	133789.596450	57.992897
2522.220303	133641.356390	57.997901
2521.407242	133471.179662	58.002906
2521.318301	133318.063137	58.007911
2520.436932	133196.372164	58.012916
2519.912665	133086.971970	58.017921
2518.728805	132924.046907	58.022925
2518.706502	132775.635345	58.027930
2517.489937	132656.654606	58.032935
2516.826663	132491.540925	58.037940
2516.230999	132354.667177	58.042945
2515.488526	132236.413301	58.047949
2514.978337	132062.576883	58.052954
2514.097080	131958.293045	58.057959
2513.539894	131807.532533	58.062964
2513.183438	131677.127552	58.067969
2512.717651	131534.191086	58.072973
2512.109573	131376.772478	58.077978
2511.352273	131252.263104	58.082983
2510.603727	131110.123007	58.087988
2510.019360	130944.929652	58.092993
2509.227047	130823.476106	58.097997
2508.928274	130664.462879	58.103002
2508.093067	130522.987266	58.108007
2507.131736	130388.810212	58.113012
2506.837505	130209.171918	58.118017
2506.009468	130103.743422	58.123021
2505.108837	129937.640848	58.128026
2504.368360	129800.840591	58.133031
2504.307850	129660.326151	58.138036
2503.290932	129509.142826	58.143041
2502.496188	129368.936747	58.148045
2502.145837	129211.210062	58.153050
2501.231068	129104.084499	58.158055
2500.569536	128927.103646	58.163060
2499.928939	128802.180291	58.168065
2499.268838	128653.675705	58.173069
2498.829434	128502.114229	58.178074
2497.933437	128387.215792	58.183079
2497.432844	128225.225805	58.188084
2496.707681	128077.801460	58.193089
2495.851595	127925.585283	58.198093
2495.453147	127793.884316	58.203098
2494.684151	127639.128596	58.208103
2493.888427	127491.121681	58.213108
2493.887654	127371.386601	58.218113
2492.941581	127195.516071	58.223117
2492.199400	127073.296340	58.228122
2491.172319	126903.917424	58.233127
2490.956509	126784.942878	58.238132
2490.269888	126619.816947	58.243137
2489.399801	126476.386466	58.248141
2489.016195	126331.609687	58.253146
2487.973338	126177.426337	58.258151
2487.501849	126053.923735	58.263156
2486.797700	125892.259215	58.268161
2486.081279	125752.948153	58.273165
2485.324198	125607.739165	58.278170
2484.779973	125466.319629	58.283175
2484.084771	125312.378175	58.288180
2483.621641	125177.487270	58.293185
2482.291172	125026.606986	58.298189
2482.099602	124885.312380	58.303194
2481.352388	124745.820913	58.308199
2481.085727	124589.542592	58.313204
2479.931469	124468.618998	58.318209
2479.470863	124305.553936	58.323213
2478.835851	124149.222277	58.328218
2478.164621	124043.398660	58.333223
2477.195125	123885.089821	58.338228
2476.882319	123729.992066	58.343233
2476.088825	123603.796225	58.348237
2475.531571	123447.811889	58.353242
2475.235782	123314.440293	58.358247
2474.275158	123164.603908	58.363252
2473.526353	123012.601547	58.368257
2472.480847	122876.392377	58.373261
2471.974886	122730.219531	58.378266
2471.539553	122579.541316	58.383271
2470.436045	122431.864925	58.388276
2470.169815	122302.480771	58.393281
2469.599691	122178.541850	58.398285
2469.185455	122007.788826	58.403290
2468.419124	121880.517592	58.408295
2467.738353	121719.242809	58.413300
2467.208939	121564.890383	58.418305
2466.795482	121441.095155	58.423309
2466.002103	121264.832999	58.428314
2464.986023	121147.889504	58.433319
2464.492272	120975.771799	58.438324
2463.913716	120833.404643	58.443329
2463.020402	120700.471067	58.448333
2462.696656	120530.144977	58.453338
2461.676358	120407.136441	58.458343
2461.418992	120223.736993	58.463348
2460.806327	120118.700643	58.468353
2459.952756	119930.585793	58.473357
2459.449124	119799.099557	58.478362
2458.421293	119635.677103	58.483367
2458.070670	119476.725299	58.488372
2457.348094	119321.394684	58.493377
2456.353369	119187.831050	58.498381
2455.396037	119030.120798	58.503386
2455.350487	118899.525047	58.508391
2454.551813	118725.159883	58.513396
2453.565171	118606.883727	58.518401
2453.013638	118427.409443	58.523405
2452.428741	118313.489038	58.528410
2451.652627	118141.219018	58.533415
2451.002733	117993.933819	58.538420
2450.820120	117877.920298	58.543425
2449.970157	117697.577989	58.548429
2449.324147	117562.545618	58.553434
2448.756100	117436.248573	58.558439
2448.125482	117240.411986	58.563444
2447.468463	117129.574124	58.568449
2446.469365	116960.273578	58.573453
2446.152963	116790.155019	58.578458
2444.869535	116675.495717	58.583463
2444.462563	116510.763277	58.588468
2444.339928	116367.631188	58.593473
2443.490361	116185.515880	58.598477
2442.887116	116078.850568	58.603482
2442.025213	115922.940560	58.608487
2441.539571	115754.950322	58.613492
2440.888128	115616.977674	58.618497
2439.713813	115472.049733	58.623501
2439.660217	115294.308385	58.628506
2438.770647	115177.232312	58.633511
2438.184872	114999.145804	58.638516
2437.648190	114872.900939	58.643521
2436.412916	114687.918905	58.648525
2435.934531	114566.458245	58.653530
2435.677713	114400.465383	58.658535
2434.670265	114242.722848	58.663540
2434.175758	114113.834838	58.668545
2433.208444	113957.160336	58.673549
2432.677757	113803.749603	58.678554
2432.068171	113649.920744	58.683559
2431.176068	113507.402837	58.688564
2430.785735	113371.279697	58.693569
2430.102038	113211.042559	58.698573
2429.420079	113080.044461	58.703578
2429.106600	112908.085721	58.708583
2427.977426	112766.168117	58.713588
2427.601795	112615.285013	58.718593
2426.469066	112465.030554	58.723597
2426.845621	112295.974814	58.728602
2425.685278	112172.577693	58.733607
2424.969929	111989.748054	58.738612
2424.454564	111858.793443	58.743617
2423.559154	111703.257684	58.748621
2422.898034	111541.371389	58.753626
2422.213333	111392.727780	58.758631
2421.528072	111239.941200	58.763636
2420.958047	111099.987921	58.768641
2420.111133	110952.235738	58.773645
2419.385205	110781.740557	58.778650
2418.690390	110649.703932	58.783655
2418.253136	110496.654196	58.788660
2417.702292	110332.664238	58.793665
2416.945662	110212.461977	58.798669
2416.474834	110028.453194	58.803674
2415.557795	109883.294922	58.808679
2414.877322	109731.437090	58.813684
2414.576970	109564.652212	58.818689
2413.399607	109450.358345	58.823693
2413.227777	109274.392084	58.828698
2412.441052	109117.370631	58.833703
2411.923719	108957.001512	58.838708
2411.575515	108837.122000	58.843713
2410.572884	108653.036575	58.848717
2409.887054	108508.719153	58.853722
2409.081392	108361.058590	58.858727
2408.521415	108183.492951	58.863732
2407.884803	108042.082968	58.868737
2407.221649	107893.419160	58.873741
2406.641790	107722.877798	58.878746
2405.977171	107573.321531	58.883751
2404.747897	107440.359148	58.888756
2404.758010	107260.489149	58.893761
2403.946896	107101.156032	58.898765
2403.215603	106946.449443	58.903770
2402.417116	106807.356533	58.908775
2401.786507	106643.163047	58.913780
2401.137251	106509.726824	58.918785
2400.862365	106331.285782	58.923789
2399.964483	106199.768749	58.928794
2399.410309	106015.359557	58.933799
2398.292872	105884.830765	58.938804
2398.147750	105692.187339	58.943809
2397.241983	105585.767744	58.948813
2397.005145	105387.799210	58.953818
2395.847330	105264.766721	58.958823
2395.113339	105082.372726	58.963828
2394.832825	104958.086119	58.968833
2393.553332	104790.207976	58.973837
2393.140075	104634.691939	58.978842
2392.727419	104470.148959	58.983847
2392.159591	104337.092655	58.988852
2391.212799	104159.859276	58.993857
2390.753965	104030.942843	58.998861
2390.479026	103848.257180	59.003866
2389.383078	103720.902591	59.008871
2388.479404	103530.217730	59.013876
2388.293864	103354.500117	59.018881
2387.332550	103246.164950	59.023885
2386.824851	103077.009350	59.028890
2386.437037	102881.737465	59.033895
2385.314191	102772.085209	59.038900
2384.854988	102585.055013	59.043905
2383.738263	102466.775732	59.048909
2383.681526	102262.055145	59.053914
2382.797534	102148.422192	59.058919
2381.791254	101983.997069	59.063924
2381.974496	101792.291292	59.068929
2380.897660	101640.471679	59.073933
2380.528996	101475.555753	59.078938
2379.509581	101312.951673	59.083943
2378.629394	101178.611677	59.088948
2377.962452	101046.572990	59.093953
2377.467124	100859.993706	59.098957
2376.591120	100716.216939	59.103962
2376.174695	100569.355182	59.108967
2375.317690	100411.171914	59.113972
2375.053031	100249.832091	59.118977
2373.905654	100109.438598	59.123981
2373.841162	99922.113517	59.128986
2372.931126	99796.844107	59.133991
2372.594836	99606.653255	59.138996
2371.550107	99483.760132	59.144001
2370.715687	99298.281123	59.149005
2370.171203	99169.373467	59.154010
2369.532156	98978.284397	59.159015
2368.741973	98867.564020	59.164020
2368.084002	98671.438045	59.169025
2367.051823	98548.325955	59.174029
2366.936234	98365.994289	59.179034
2366.067147	98232.468891	59.184039
2365.603305	98061.345075	59.189044
2364.759309	97918.544804	59.194049
2364.337273	97750.283486	59.199053
2363.770244	97593.760755	59.204058
2362.914657	97439.193895	59.209063
2362.159626	97280.901906	59.214068
2361.753221	97122.695274	59.219073
2360.806319	96984.737289	59.224077
2360.585981	96793.777720	59.229082
2359.920316	96669.336577	59.234087
2358.979156	96482.736798	59.239092
2358.434821	96338.706651	59.244097
2357.638218	96193.493420	59.249101
2357.130240	96013.120080	59.254106
2356.414870	95853.493646	59.259111
2355.597048	95701.114284	59.264116
2355.328963	95550.050325	59.269121
2354.510096	95401.763617	59.274125
2353.548749	95229.585892	59.279130
2353.078172	95071.251615	59.284135
2352.318795	94902.164477	59.289140
2351.683621	94768.438548	59.294145
2350.941950	94599.388939	59.299149
2350.650253	94447.904923	59.304154
2349.796616	94289.288134	59.309159
2349.107202	94127.247446	59.314164
2348.216401	93968.759316	59.319169
2347.651843	93811.121050	59.324173
2346.895362	93657.059096	59.329178
2346.357862	93505.886787	59.334183
2345.631718	93350.205139	59.339188
2345.240207	93200.127809	59.344193
2344.376899	93034.996475	59.349197
2344.254816	92869.438128	59.354202
2343.100303	92725.959192	59.359207
2342.463683	92571.403857	59.364212
2342.240701	92405.757180	59.369217
2341.502216	92245.088627	59.374221
2340.784509	92067.931848	59.379226
2339.950316	91908.688581	59.384231
2339.225942	91754.133862	59.389236
2338.621994	91590.069151	59.394241
2337.690045	91436.614811	59.399245
2336.854829	91281.453270	59.404250
2336.611955	91114.126525	59.409255
2335.614226	90953.603622	59.414260
2335.259485	90799.694463	59.419265
2334.557213	90663.518523	59.424269
2333.750143	90495.715329	59.429274
2333.174928	90335.611830	59.434279
2332.610298	90172.584966	59.439284
2332.036337	90008.717553	59.444289
2330.999757	89860.920966	59.449293
2330.778905	89713.319379	59.454298
2330.343044	89533.760856	59.459303
2329.118970	89392.254839	59.464308
2328.841174	89212.946523	59.469313
2328.150796	89063.807104	59.474317
2327.570464	88888.404125	59.479322
2326.849518	88753.751987	59.484327
2326.324782	88565.916711	59.489332
2325.415953	88402.558305	59.494337
2324.616285	88261.100158	59.499341
2323.993299	88075.440224	59.504346
2323.141795	87950.107722	59.509351
2322.498926	87757.131434	59.514356
2322.233078	87630.294203	59.519361
2321.328277	87452.767207	59.524365
2320.769143	87292.747036	59.529370
2320.376075	87138.312065	59.534375
2319.342135	86983.555098	59.539380
2319.306608	86822.384057	59.544385
2318.303156	86652.036374	59.549389
2317.539074	86484.828016	59.554394
2317.103951	86326.088590	59.559399
2316.428008	86163.306162	59.564404
2315.754503	85987.472524	59.569409
2314.714662	85834.854724	59.574413
2314.413442	85668.010416	59.579418
2313.577047	85508.034890	59.584423
2312.860179	85342.374692	59.589428
2312.405445	85166.563852	59.594433
2311.345750	85029.092009	59.599437
2311.020917	84855.595803	59.604442
2310.404368	84700.256778	59.609447
2309.685928	84528.270881	59.614452
2308.935910	84365.437908	59.619457
2308.476356	84212.562277	59.624461
2307.704423	84042.997441	59.629466
2306.948170	83871.529961	59.634471
2305.959233	83719.305971	59.639476
2305.677564	83539.735240	59.644481
2304.635438	83391.344051	59.649485
2304.123664	83240.220435	59.654490
2303.727309	83084.623874	59.659495
2303.056608	82914.025296	59.664500
2302.276891	82749.447535	59.669505
2301.692130	82596.578147	59.674509
2301.137859	82429.349549	59.679514
2300.106605	82273.910394	59.684519
2299.381728	82118.024523	59.689524
2299.413868	81928.011046	59.694529
2298.177427	81783.895722	59.699533
2297.447440	81613.925576	59.704538
2296.788490	81458.661612	59.709543
2295.970261	81303.195910	59.714548
2295.429563	81145.405832	59.719553
2294.612184	80987.420004	59.724557
2294.467023	80823.263809	59.729562
2293.461174	80667.496734	59.734567
2292.750606	80518.705819	59.739572
2292.150216	80358.389903	59.744577
2291.801181	80198.574034	59.749581
2290.885183	80025.908686	59.754586
2290.217429	79869.067374	59.759591
2289.619808	79718.933494	59.764596
2289.262907	79564.808187	59.769601
2288.495821	79404.957028	59.774605
2287.974002	79230.480466	59.779610
2287.333468	79071.118788	59.784615
2286.656580	78902.562952	59.789620
2285.885448	78742.628867	59.794625
2285.522529	78575.800234	59.799629
2284.680976	78410.867508	59.804634
2283.970852	78242.144940	59.809639
2283.195987	78079.783334	59.814644
2282.451665	77916.708476	59.819649
2281.585611	77754.611042	59.824653
2281.250715	77590.903565	59.829658
2280.833984	77422.635479	59.834663
2279.727220	77280.165895	59.839668
2279.442931	77098.452690	59.844673
2278.305901	76940.079779	59.849677
2277.743594	76767.119672	59.854682
2277.264763	76616.831296	59.859687
2276.558501	76441.083533	59.864692
2276.079695	76284.524854	59.869697
2275.250025	76137.267291	59.874701
2274.909226	75951.961771	59.879706
2274.222727	75785.606468	59.884711
2273.524130	75631.349621	59.889716
2272.823907	75457.098373	59.894721
2271.779977	75306.282104	59.899725
2271.477027	75122.929601	59.904730
2270.690925	74964.624207	59.909735
2269.747573	74811.831637	59.914740
2269.655748	74637.452973	59.919745
2268.343609	74468.116020	59.924750
2267.996133	74321.669544	59.929754
2267.504083	74144.678735	59.934759
2266.503387	73979.598251	59.939764
2266.088138	73821.033992	59.944769
2265.502192	73656.536594	59.949774
2264.725199	73493.230189	59.954778
2263.947332	73320.650611	59.959783
2263.333774	73163.687797	59.964788
2262.846074	73010.716338	59.969793
2261.636137	72826.413721	59.974798
2261.058342	72680.801331	59.979802
2260.686302	72515.455875	59.984807
2259.847556	72345.935142	59.989812
2259.546182	72182.095275	59.994817
2258.782923	72038.601147	59.999822
2258.044328	71860.865198	60.004826
2257.339337	71694.616515	60.009831
2256.681742	71547.656815	60.014836
2256.341745	71373.719776	60.019841
2255.449083	71205.452585	60.024846
2254.698082	71040.933335	60.029850
2254.079721	70882.595758	60.034855
2253.581544	70722.479453	60.039860
2252.880559	70550.830262	60.044865
2252.128485	70381.724350	60.049870
2251.806595	70222.179568	60.054874
2250.829862	70067.173811	60.059879
2250.118190	69902.385473	60.064884
2249.667037	69725.953327	60.069889
2248.839094	69563.276496	60.074894
2248.477372	69390.481532	60.079898
2248.149819	69232.674844	60.084903
2246.887163	69062.356522	60.089908
2246.159714	68890.941404	60.094913
2245.343437	68724.355465	60.099918
2245.128541	68555.585473	60.104922
2244.206597	68390.646882	60.109927
2243.438551	68220.878151	60.114932
2243.185554	68051.200213	60.119937
2242.270391	67899.096281	60.124942
2241.720103	67738.170318	60.129946
2241.021277	67567.110650	60.134951
2240.450771	67399.395085	60.139956
2239.429355	67240.498612	60.144961
2238.657614	67068.894421	60.149966
2238.097645	66903.949052	60.154970
2237.609497	66748.094247	60.159975
2236.437635	66581.997908	60.164980
2236.196305	66405.904564	60.169985
2235.601427	66254.570204	60.174990
2235.006621	66096.270932	60.179994
2234.493756	65919.873625	60.184999
2233.872401	65762.509056	60.190004
2233.362343	65596.214926	60.195009
2232.415157	65430.371525	60.200014
2231.935376	65250.653669	60.205018
2231.448656	65088.938650	60.210023
2230.668081	64918.953971	60.215028
2230.180375	64738.779905	60.220033
2229.536373	64573.348596	60.225038
2228.546405	64404.383210	60.230042
2227.947141	64237.304497	60.235047
2227.335428	64060.398580	60.240052
2226.624528	63898.418915	60.245057
2225.935204	63735.569717	60.250062
2225.401796	63551.070342	60.255066
2224.463174	63387.326537	60.260071
2223.410851	63209.358673	60.265076
2223.096366	63046.231144	60.270081
2222.434137	62879.164845	60.275086
2221.822515	62738.973182	60.280090
2221.086753	62540.491026	60.285095
2220.273226	62373.142939	60.290100
2219.857843	62218.196774	60.295105
2219.068397	62063.649947	60.300110
2218.500955	61894.595557	60.305114
2218.105940	61725.641958	60.310119
2217.040339	61565.390981	60.315124
2216.586391	61383.445307	60.320129
2215.849562	61219.694597	60.325134
2215.414960	61060.215205	60.330138
2214.816842	60888.395345	60.335143
2213.945321	60718.548220	60.340148
2213.603543	60550.043070	60.345153
2212.788442	60373.314700	60.350158
2212.312922	60204.124813	60.355162
2211.729390	60032.687166	60.360167
2210.635146	59862.288042	60.365172
2210.290445	59690.746008	60.370177
2209.338684	59523.404081	60.375182
2208.654917	59355.422908	60.380186
2208.086295	59180.135416	60.385191
2207.087792	59020.648904	60.390196
2206.564111	58839.027054	60.395201
2205.776960	58674.290590	60.400206
2204.796754	58503.328741	60.405210
2204.551962	58347.586746	60.410215
2203.801867	58202.190569	60.415220
2203.281148	58015.483687	60.420225
2202.901192	57856.861737	60.425230
2201.849987	57678.135974	60.430234
2201.343290	57517.596898	60.435239
2200.552679	57355.664205	60.440244
2200.213335	57177.934923	60.445249
2199.629450	57013.370888	60.450254
2198.832525	56841.692721	60.455258
2198.308420	56670.134283	60.460263
2197.312052	56505.051565	60.465268
2196.858031	56339.570986	60.470273
2196.053729	56175.983007	60.475278
2195.398549	56006.600407	60.480282
2194.984665	55838.317213	60.485287
2193.871964	55661.209455	60.490292
2193.529938	55497.557361	60.495297
2192.392691	55328.975864	60.500302
2192.122815	55156.416555	60.505306
2191.706707	54995.264884	60.510311
2191.073805	54827.715591	60.515316
2190.464818	54643.268933	60.520321
2189.734359	54479.494541	60.525326
2189.063884	54304.661980	60.530330
2188.637830	54141.763179	60.535335
2187.830972	53974.657532	60.540340
2187.167772	53786.949879	60.545345
2186.339891	53618.040856	60.550350
2185.761814	53437.313235	60.555354
2184.942362	53274.354885	60.560359
2184.304673	53099.155349	60.565364
2184.239378	52928.448425	60.570369
2183.051464	52753.845784	60.575374
2182.131611	52584.657234	60.580378
2181.587440	52412.455421	60.585383
2180.930590	52250.106998	60.590388
2180.849572	52070.181137	60.595393
2179.728275	51901.325208	60.600398
2179.361070	51720.407286	60.605402
2178.755632	51544.407753	60.610407
2178.032381	51377.316022	60.615412
2177.095209	51194.525866	60.620417
2176.538494	51022.041942	60.625422
2175.658658	50836.576061	60.630426
2174.793352	50668.387156	60.635431
2174.011642	50516.957587	60.640436
2173.626436	50343.396299	60.645441
2172.614664	50165.826466	60.650446
2172.282092	50004.180891	60.655450
2171.807406	49832.150992	60.660455
2170.766329	49665.340793	60.665460
2170.351467	49499.321776	60.670465
2169.649870	49335.668667	60.675470
2168.578722	49157.713366	60.680474
2168.231713	48993.646513	60.685479
2167.586108	48829.973359	60.690484
2167.201928	48656.143631	60.695489
2166.480864	48497.078800	60.700494
2165.588576	48326.863250	60.705498
2165.089515	48158.146474	60.710503
2164.354655	47988.209721	60.715508
2163.815176	47814.030133	60.720513
2163.004417	47648.129203	60.725518
2162.488833	47482.021681	60.730522
2161.823328	47302.416928	60.735527
2161.478052	47141.375143	60.740532
2160.827652	46964.456949	60.745537
2159.939328	46781.448225	60.750542
2159.170670	46616.015306	60.755546
2158.423262	46445.203437	60.760551
2157.932856	46269.661744	60.765556
2157.342355	46101.769904	60.770561
2156.595236	45932.408453	60.775566
2156.201466	45755.097990	60.780570
2155.845460	45580.421159	60.785575
2154.849515	45414.656090	60.790580
2154.326768	45232.035687	60.795585
2153.248442	45057.077004	60.800590
2152.580793	44880.811967	60.805594
2152.021985	44706.713712	60.810599
2151.487181	44539.890705	60.815604
2150.699999	44367.707536	60.820609
2149.775328	44192.518100	60.825614
2149.384323	44013.555032	60.830618
2148.484211	43837.950977	60.835623
2148.104550	43671.108529	60.840628
2147.484509	43505.668853	60.845633
2146.606070	43334.655227	60.850638
2145.843507	43155.769442	60.855642
2145.613163	42985.247819	60.860647
2144.681386	42806.553774	60.865652
2144.033829	42627.357947	60.870657
2143.080687	42473.574088	60.875662
2142.767325	42297.943169	60.880666
2142.546620	42122.805295	60.885671
2141.310828	41951.602757	60.890676
2140.832686	41773.815077	60.895681
2139.924989	41604.201948	60.900686
2139.177178	41429.218002	60.905690
2139.118301	41249.509906	60.910695
2138.092719	41080.881921	60.915700
2137.556363	40907.795428	60.920705
2136.875071	40722.433579	60.925710
2136.068900	40554.251845	60.930714
2135.728002	40377.370662	60.935719
2134.932291	40212.676639	60.940724
2134.451646	40023.769771	60.945729
2133.656314	39865.372699	60.950734
2132.899542	39680.348729	60.955738
2132.501422	39499.806978	60.960743
2131.567926	39335.731371	60.965748
2130.963562	39147.935146	60.970753
2129.710290	38986.582107	60.975758
2129.460998	38809.310612	60.980762
2129.249028	38644.055416	60.985767
2127.896572	38473.448464	60.990772
2127.565563	38287.864670	60.995777
2126.784068	38121.043549	61.000782
2126.093619	37940.937807	61.005786
2125.822527	37764.303504	61.010791
2124.972144	37602.779592	61.015796
2124.480805	37409.581867	61.020801
2123.679869	37250.438729	61.025806
2123.147440	37067.155901	61.030810
2122.497322	36899.523032	61.035815
2121.490234	36734.271978	61.040820
2121.036334	36546.700461	61.045825
2120.705160	36365.767398	61.050830
2119.205235	36199.374848	61.055834
2119.028452	36027.589806	61.060839
2118.373652	35857.741075	61.065844
2117.617302	35675.360858	61.070849
2116.978745	35510.208793	61.075854
2116.324328	35326.088719	61.080858
2115.809907	35152.351102	61.085863
2114.850198	34980.843259	61.090868
2114.439384	34810.302659	61.095873
2113.588908	34632.849684	61.100878
2113.156427	34464.609244	61.105882
2112.418588	34278.543196	61.110887
2111.463329	34113.426752	61.115892
2110.776339	33932.597013	61.120897
2110.479524	33761.358448	61.125902
2109.789897	33595.751443	61.130906
2109.038553	33417.097825	61.135911
2108.373795	33257.446418	61.140916
2107.879130	33067.548434	61.145921
2106.987205	32886.296433	61.150926
2106.098245	32726.113671	61.155930
2105.785425	32560.454065	61.160935
2104.934378	32377.116847	61.165940
2104.559075	32210.789592	61.170945
2103.874730	32042.847546	61.175950
2103.054741	31851.111046	61.180954
2102.833798	31677.745628	61.185959
2101.594797	31497.115422	61.190964
2100.798413	31321.362694	61.195969
2100.440013	31152.505794	61.200974
2099.615353	30990.321410	61.205978
2098.926372	30822.596384	61.210983
2098.047795	30666.099322	61.215988
2098.013881	30480.438364	61.220993
2097.182888	30302.328847	61.225998
2095.981078	30138.348331	61.231002
2095.467295	29956.948522	61.236007
2095.176229	29797.017006	61.241012
2094.489875	29617.879243	61.246017
2094.036757	29441.779385	61.251022
2093.181470	29276.224759	61.256026
2092.722734	29096.184498	61.261031
2091.508739	28920.830318	61.266036
2091.218955	28750.876671	61.271041
2090.308546	28585.378895	61.276046
2089.859196	28408.585003	61.281050
2089.449895	28234.668246	61.286055
2088.374339	28065.198750	61.291060
2087.694963	27896.740828	61.296065
2086.929448	27726.088246	61.301070
2086.404104	27545.453318	61.306074
2085.499110	27379.288497	61.311079
2084.543525	27216.889953	61.316084
2084.441456	27048.538818	61.321089
2083.607446	26890.736167	61.326094
2082.800655	26706.655506	61.331098
2082.485493	26538.435124	61.336103
2081.803878	26375.297849	61.341108
2081.303265	26209.568222	61.346113
2080.379625	26037.453219	61.351118
2079.687005	25867.957084	61.356122
2079.193928	25691.448642	61.361127
2078.147244	25525.110610	61.366132
2077.844910	25353.679110	61.371137
2077.037039	25185.007714	61.376142
2076.265771	25025.680502	61.381146
2076.037926	24849.800252	61.386151
2074.949562	24685.604314	61.391156
2074.212507	24521.187686	61.396161
2073.356892	24350.758950	61.401166
2072.813630	24186.166553	61.406170
2072.146160	24020.381010	61.411175
2071.135860	23864.431879	61.416180
2070.931098	23690.977959	61.421185
2070.329606	23533.645272	61.426190
2069.537187	23374.664821	61.431194
2068.860149	23194.749676	61.436199
2068.230475	23042.131878	61.441204
2067.514677	22879.842704	61.446209
2066.690323	22720.688302	61.451214
2066.306430	22557.015284	61.456218
2065.337122	22388.874458	61.461223
2064.789009	22232.943018	61.466228
2064.007482	22063.750147	61.471233
2063.387655	21909.962028	61.476238
2062.486052	21750.783839	61.481242
2061.969238	21591.680421	61.486247
2061.262615	21431.748888	61.491252
2060.945808	21275.478309	61.496257
2059.902268	21120.211270	61.501262
2059.173669	20965.564527	61.506266
2058.522211	20813.646753	61.511271
2057.607749	20657.192521	61.516276
2057.249152	20495.739241	61.521281
2056.547612	20343.101285	61.526286
2055.350543	20192.529053	61.531290
2054.939821	20044.035785	61.536295
2054.341939	19901.303347	61.541300
2053.752160	19737.577790	61.546305
2053.086067	19598.541079	61.551310
2052.169909	19442.232260	61.556314
2051.990509	19285.863742	61.561319
2050.930260	19146.072170	61.566324
2050.544494	18982.841987	61.571329
2049.792302	18844.105111	61.576334
2049.001465	18688.559565	61.581338
2048.607808	18534.804129	61.586343
2047.551792	18383.040835	61.591348
2047.146399	18241.471997	61.596353
2046.225050	18086.874407	61.601358
2045.830663	17934.241617	61.606362
2045.204791	17790.395797	61.611367
2044.081902	17654.047561	61.616372
2043.488731	17506.760258	61.621377
2042.767352	17353.796889	61.626382
2041.803520	17211.302844	61.631386
2041.417847	17063.557410	61.636391
2040.426333	16943.715214	61.641396
2039.761200	16800.853518	61.646401
2039.052263	16676.412121	61.651406
2038.445580	16537.804365	61.656410
2037.420660	16398.859111	61.661415
2036.553993	16270.523129	61.666420
2035.741588	16145.306809	61.671425
2035.066147	16028.694974	61.676430
2033.894363	15927.962964	61.681434
2033.060070	15801.683421	61.686439
2032.253833	15709.508565	61.691444
2031.426611	15584.988977	61.696449
2030.563317	15488.354562	61.701454
2029.308932	15404.473262	61.706458
2029.028736	15308.108331	61.711463
2027.797423	15198.013587	61.716468
2027.096140	15113.773312	61.721473
2026.470878	15035.174485	61.726478
2025.565546	14947.481715	61.731482
2024.897821	14873.447915	61.736487
2024.240491	14793.632693	61.741492
2023.631452	14709.781616	61.746497
2022.591552	14646.656490	61.751502
2021.633892	14568.542861	61.756506
2021.197125	14502.061953	61.761511
2020.620866	14437.690346	61.766516
2019.960409	14370.121475	61.771521
2019.205472	14306.214817	61.776526
2018.313560	14227.536574	61.781530
2017.587999	14157.121671	61.786535
2016.890132	14101.422859	61.791540
2016.577750	14031.453868	61.796545
2015.889174	13977.253990	61.801550
2014.822079	13916.197363	61.806554
2014.451140	13844.667252	61.811559
2013.698578	13786.552224	61.816564
2013.410934	13727.686395	61.821569
2012.596068	13663.102989	61.826574
2011.905080	13592.663601	61.831578
2011.230217	13525.818106	61.836583
2010.195119	13468.647203	61.841588
2009.999216	13415.881782	61.846593
2009.058650	13366.808821	61.851598
2008.312199	13305.086733	61.856602
2007.799146	13244.669803	61.861607
2007.109386	13187.975949	61.866612
2006.515617	13131.555503	61.871617
2006.154803	13075.856264	61.876622
2005.650170	13009.545027	61.881626
2004.962393	12930.561230	61.886631
2004.134755	12884.788340	61.891636
2003.752983	12813.532695	61.896641
2003.112208	12746.164290	61.901646
2002.435057	12688.461794	61.906650
2001.704044	12617.731431	61.911655
2000.990073	12564.147940	61.916660
2000.365048	12490.994937	61.921665
1999.598194	12436.604151	61.926670
1998.778862	12375.807247	61.931674
1998.181554	12301.769917	61.936679
1997.403018	12260.740922	61.941684
1996.784818	12189.103166	61.946689
1996.491844	12141.489752	61.951694
1995.530601	12094.008002	61.956698
1995.357729	12018.838231	61.961703
1994.449795	11954.729893	61.966708
1993.748695	11901.629818	61.971713
1993.329562	11837.845444	61.976718
1992.800787	11762.118741	61.981722
1992.078381	11706.448379	61.986727
1991.017702	11643.441107	61.991732
1990.859647	11583.189464	61.996737
1990.064519	11513.199976	62.001742
1989.198400	11454.277171	62.006746
1989.097370	11376.736544	62.011751
1987.755730	11319.836729	62.016756
1987.012575	11253.312415	62.021761
1986.412478	11204.753534	62.026766
1985.961575	11148.053069	62.031770
1985.143670	11083.982661	62.036775
1984.277129	11028.240229	62.041780
1983.831632	10959.625968	62.046785
1983.268874	10911.170597	62.051790
1982.438581	10846.595621	62.056794
1981.904604	10786.293593	62.061799
1981.458872	10729.253022	62.066804
1980.587828	10672.901129	62.071809
1980.244846	10614.579888	62.076814
1979.385378	10548.794356	62.081818
1978.935003	10478.880793	62.086823
1977.944430	10419.384903	62.091828
1977.439665	10360.919898	62.096833
1976.777706	10307.798705	62.101838
1975.842938	10250.929879	62.106842
1975.126361	10189.686786	62.111847
1974.665681	10132.921075	62.116852
1974.334909	10066.088014	62.121857
1973.450603	10014.338508	62.126862
1973.147705	9956.945634	62.131866
1972.583089	9882.742775	62.136871
1971.723262	9813.843667	62.141876
1971.286722	9764.719868	62.146881
1970.454059	9696.384650	62.151886
1969.677674	9629.316958	62.156890
1969.216411	9557.904061	62.161895
1968.022037	9504.774358	62.166900
1967.616445	9434.925993	62.171905
1967.030329	9382.131341	62.176910
1965.949448	9318.921235	62.181914
1965.542320	9263.859165	62.186919
1964.627215	9216.538147	62.191924
1964.143515	9148.024203	62.196929
1963.341389	9092.004972	62.201934
1962.762823	9048.342610	62.206938
1962.289771	8976.778931	62.211943
1961.284144	8916.631456	62.216948
1961.310879	8855.950747	62.221953
1960.574774	8800.765089	62.226958
1959.676296	8738.264547	62.231962
1959.125653	8663.524700	62.236967
1958.050909	8623.484157	62.241972
1957.357818	8560.421216	62.246977
1956.948559	8499.916867	62.251982
1956.184431	8433.699473	62.256986
1955.502424	8381.244261	62.261991
1954.643612	8332.768081	62.266996
1954.403729	8275.202816	62.272001
1953.461811	8218.832353	62.277006
1952.906660	8157.810976	62.282010
1952.619055	8099.734087	62.287015
1951.680236	8048.646920	62.292020
1951.072896	7982.061902	62.297025
1950.377165	7926.791025	62.302030
1949.578714	7863.467308	62.307034
1949.282390	7809.277327	62.312039
1948.496633	7747.892699	62.317044
1947.904123	7686.869712	62.322049
1947.334615	7629.589606	62.327054
1946.393853	7565.943436	62.332058
1946.042230	7501.569390	62.337063
1945.079203	7464.827803	62.342068
1944.005972	7402.752658	62.347073
1943.396102	7338.813549	62.352078
1942.682960	7283.223611	62.357082
1942.252369	7227.107840	62.362087
1941.292272	7182.233591	62.367092
1941.076339	7122.031905	62.372097
1940.469601	7066.438509	62.377102
1939.509396	7013.034411	62.382106
1939.455872	6947.620339	62.387111
1938.562994	6899.263886	62.392116
1937.547646	6836.700742	62.397121
1937.009881	6780.561862	62.402126
1936.655562	6733.383348	62.407130
1936.129858	6673.912602	62.412135
1935.283812	6616.868822	62.417140
1934.736809	6561.050127	62.422145
1933.778692	6506.414628	62.427150
1932.881660	6447.609532	62.432154
1932.921508	6377.642844	62.437159
1931.845892	6327.426535	62.442164
1931.249760	6274.500528	62.447169
1930.561764	6212.652388	62.452174
1929.920244	6153.203693	62.457178
1929.061972	6102.298961	62.462183
1928.445234	6047.009132	62.467188
1928.060739	5980.869393	62.472193
1927.109129	5933.874215	62.477198
1926.423115	5876.524718	62.482202
1926.006401	5822.494394	62.487207
1925.454083	5767.323163	62.492212
1924.527200	5705.917331	62.497217
1924.161000	5641.322953	62.502222
1923.362597	5594.978128	62.507226
1922.717658	5536.408756	62.512231
1921.768673	5480.518341	62.517236
1921.510337	5422.390479	62.522241
1920.374053	5364.051228	62.527246
1919.655661	5318.476999	62.532250
1919.307615	5252.535857	62.537255
1918.635889	5194.760036	62.542260
1917.757224	5149.354532	62.547265
1917.247313	5096.567337	62.552270
1916.381315	5031.361681	62.557274
1916.094716	4973.139117	62.562279
1915.312382	4940.480399	62.567284
1914.794373	4870.730849	62.572289
1913.927677	4817.187345	62.577294
1913.178729	4761.340464	62.582298
1912.565050	4714.599972	62.587303
1911.875567	4665.737440	62.592308
1911.384666	4605.961107	62.597313
1910.475574	4552.598021	62.602318
1910.172671	4499.189373	62.607322
1909.418555	4432.540290	62.612327
1908.820070	4386.449884	62.617332
1908.283416	4318.235959	62.622337
1907.440922	4261.066649	62.627342
1906.781888	4210.909730	62.632346
1906.212824	4156.972787	62.637351
1905.446268	4107.962668	62.642356
1904.769395	4041.297576	62.647361
1903.876141	3992.006688	62.652366
1902.980341	3939.737597	62.657370
1902.860215	3877.591432	62.662375
1901.920087	3849.565166	62.667380
1901.290395	3791.703798	62.672385
1900.682837	3720.221533	62.677390
1900.283400	3678.098626	62.682394
1899.493552	3618.392697	62.687399
1898.965499	3565.828388	62.692404
1898.262427	3513.400885	62.697409
1897.569962	3448.019347	62.702414
1896.779272	3402.680203	62.707418
1896.357447	3335.391087	62.712423
1895.387147	3300.269070	62.717428
1894.498770	3233.731920	62.722433
1893.987236	3185.412301	62.727438
1893.063018	3140.221349	62.732442
1892.773690	3081.242540	62.737447
1891.810993	3034.017880	62.742452
1891.193818	2985.886032	62.747457
1890.428720	2940.401522	62.752462
1889.972054	2889.229665	62.757466
1889.534824	2834.741986	62.762471
1888.665531	2791.610319	62.767476
1887.885063	2745.796856	62.772481
1887.534123	2686.868847	62.777486
1886.973047	2642.112292	62.782490
1886.146204	2582.592321	62.787495
1885.600269	2531.078660	62.792500
1884.737358	2472.096373	62.797505
1884.024785	2427.961483	62.802510
1883.539064	2382.899620	62.807514
1883.060840	2309.060853	62.812519
1882.216733	2274.493780	62.817524
1881.565845	2215.923623	62.822529
1880.886717	2157.845518	62.827534
1879.801504	2123.442465	62.832538
1879.234344	2066.803423	62.837543
1878.620094	2021.796201	62.842548
1878.308600	1976.548644	62.847553
1877.533916	1917.710729	62.852558
1876.523965	1870.715774	62.857562
1876.060226	1822.250352	62.862567
1875.134814	1786.525569	62.867572
1874.569517	1732.071803	62.872577
1874.168197	1677.376147	62.877582
1873.537758	1633.919021	62.882586
1873.049011	1586.659295	62.887591
1872.247756	1537.648333	62.892596
1871.481029	1489.825887	62.897601
1870.815468	1434.288368	62.902606
1869.758400	1380.382379	62.907610
1869.465480	1328.798106	62.912615
1868.675515	1295.682745	62.917620
1868.018380	1243.573095	62.922625
1867.546598	1209.830220	62.927630
1866.598399	1162.069207	62.932634
1866.409796	1099.862135	62.937639
1865.612720	1063.864072	62.942644
1864.818835	1004.998996	62.947649
1864.366432	969.902109	62.952654
1863.325947	916.451756	62.957658
1863.095491	859.819152	62.962663
1861.754770	825.259477	62.967668
1861.076121	775.323283	62.972673
1860.288122	733.084492	62.977678
1859.886334	684.766784	62.982682
1859.494073	637.565794	62.987687
1858.563021	613.672837	62.992692
1857.737853	557.489077	62.997697
1857.291222	521.148142	63.002702
1856.215703	489.144410	63.007706
1855.905320	434.213494	63.012711
1855.396360	400.889989	63.017716
1854.583114	367.723680	63.022721
1853.838336	316.657867	63.027726
1853.275193	274.633870	63.032730
1852.637168	240.336186	63.037735
1851.531798	208.214819	63.042740
1850.940849	168.530963	63.047745
1850.386242	127.275575	63.052750
1849.369463	96.539110	63.057754
1849.071528	54.494146	63.062759
1848.129816	24.472870	63.067764
1847.373436	-6.471870	63.072769
1846.804554	-36.025533	63.077774
1845.856253	-65.369089	63.082778
1845.007156	-86.418145	63.087783
1841.135164	-33.762817	63.092788
1837.921919	32.781507	63.097793
1838.640702	42.986652	63.102798
1839.589081	39.910959	63.107802
1840.620217	32.107196	63.112807
1840.596772	29.438112	63.117812
1839.883548	23.346298	63.122817
1839.169192	25.817224	63.127822
1837.675669	35.318685	63.132826
1836.851972	29.965053	63.137831
1836.022194	42.538583	63.142836
1835.305104	42.961553	63.147841
1834.894383	33.172758	63.152846
1834.139673	45.206110	63.157850
1834.411767	41.889300	63.162855
1833.570156	41.940970	63.167860
1832.671680	52.289372	63.172865
1832.492780	43.871935	63.177870
1830.965704	46.486103	63.182874
1830.405578	46.054702	63.187879
1829.803225	51.152313	63.192884
1829.217101	45.346231	63.197889
1828.844787	40.821337	63.202894
1827.850269	43.756209	63.207898
1827.130986	43.212889	63.212903
1826.340485	47.353235	63.217908
1825.490599	55.662878	63.222913
1825.788992	39.212614	63.227918
1824.870442	54.555096	63.232922
1824.161851	47.161597	63.237927
1823.481178	49.707605	63.242932
1822.715369	50.668153	63.247937
1822.654989	42.405358	63.252942
1821.002532	54.820957	63.257946
1821.264081	44.434995	63.262951
1819.845523	48.214614	63.267956
1819.390640	47.577276	63.272961
1819.699530	48.160604	63.277966
1818.198492	55.058240	63.282970
1817.330274	38.364302	63.287975
1816.559777	53.317435	63.292980
1816.515581	50.383571	63.297985
1815.581890	46.476078	63.302990
1814.666661	47.559700	63.307994
1814.615347	44.220126	63.312999
1813.435067	50.823988	63.318004
1812.775936	42.571116	63.323009
1812.874900	33.518228	63.328014
1811.314672	57.458942	63.333018
1810.635026	48.594333	63.338023
1810.694199	48.220711	63.343028
1810.121191	43.803379	63.348033
1808.802492	39.458726	63.353038
1807.916509	49.147580	63.358042
1807.377724	42.635422	63.363047
1807.236210	46.018306	63.368052
1806.627868	44.795077	63.373057
1805.664382	50.689604	63.378062
1804.581461	56.626751	63.383066
1804.801323	39.720618	63.388071
1803.862600	51.016826	63.393076
1803.210135	45.167671	63.398081
1802.988292	35.347314	63.403086
1802.023530	45.078637	63.408090
1801.706689	41.170969	63.413095
1800.866664	39.736959	63.418100
1799.853843	50.185523	63.423105
1798.875194	40.578376	63.428110
1798.441627	45.049966	63.433114
1798.160074	38.049126	63.438119
1797.150457	40.563796	63.443124
1796.427101	39.589062	63.448129
1795.587800	40.835668	63.453134
1794.601704	44.422051	63.458138
1794.994922	38.386352	63.463143
1794.357410	44.760532	63.468148
1793.284784	49.529140	63.473153
1792.680189	40.856044	63.478158
1791.788441	40.781654	63.483162
1791.139630	48.132153	63.488167
1790.661016	45.669385	63.493172
1790.220199	52.460173	63.498177
1789.835271	41.716417	63.503182
1789.010931	59.521260	63.508186
1787.828887	39.280259	63.513191
1787.181403	50.864525	63.518196
1786.362853	51.838190	63.523201
1786.108056	36.038731	63.528206
1785.799780	47.184366	63.533210
1785.145063	54.199927	63.538215
1784.113653	52.575547	63.543220
1783.586660	57.553972	63.548225
1783.299035	49.850795	63.553230
1781.645005	58.508913	63.558234
1781.598966	49.682465	63.563239
1780.500046	44.705280	63.568244
1779.576824	53.893873	63.573249
1779.693993	44.576324	63.578254
1778.971308	48.937717	63.583258
1778.228498	51.471526	63.588263
1777.194680	56.060520	63.593268
1776.619567	41.363718	63.598273
1775.999073	40.725880	63.603278
1775.328245	51.708326	63.608282
1775.254552	45.000896	63.613287
1774.852688	45.682896	63.618292
1774.103845	52.418526	63.623297
1772.930784	51.083142	63.628302
1771.865696	45.920821	63.633306
1771.334171	41.050650	63.638311
1770.625797	52.387554	63.643316
1770.117890	57.739830	63.648321
1769.641826	45.305919	63.653326
1768.803617	53.842370	63.658330
1769.051625	35.857906	63.663335
1768.215136	51.117980	63.668340
1767.073971	45.663401	63.673345
1766.132868	40.429358	63.678350
1765.243001	43.976815	63.683354
1765.066402	38.422676	63.688359
1764.246562	53.976566	63.693364
1763.937970	47.645473	63.698369
1764.105182	38.941280	63.703374
1762.647937	48.132682	63.708378
1761.628712	46.943178	63.713383
1761.026414	44.321868	63.718388
1760.443461	49.064761	63.723393
1759.921370	41.154409	63.728398
1758.914230	47.169417	63.733402
1758.762902	44.361377	63.738407
1757.559603	47.390929	63.743412
1756.372014	48.386941	63.748417
1756.479956	33.755137	63.753422
1755.998994	49.324590	63.758426
1755.142387	44.837197	63.763431
1754.635920	28.823842	63.768436
1753.990597	36.741471	63.773441
1753.403508	52.767736	63.778446
1752.725140	46.744520	63.783450
1751.951747	36.783114	63.788455
1750.851333	44.366182	63.793460
1750.204839	43.518021	63.798465
1749.766986	35.442914	63.803470
1749.344586	48.084227	63.808474
1748.829934	46.991209	63.813479
1748.302595	44.613455	63.818484
1747.037316	50.948576	63.823489
1746.448774	38.144625	63.828494
1745.367065	44.176209	63.833498
1745.275303	38.769443	63.838503
1744.677490	39.402145	63.843508
1744.218166	49.590938	63.848513
1743.940043	37.559254	63.853518
1742.726944	47.550801	63.858522
1741.854546	32.932772	63.863527
1741.151641	40.555209	63.868532
1740.500327	49.565012	63.873537
1740.044095	40.174536	63.878542
1739.355688	51.325353	63.883546
1739.122842	52.119283	63.888551
1737.710949	48.295652	63.893556
1736.811480	48.640385	63.898561
1736.162666	43.948116	63.903566
1735.608332	58.308712	63.908570
1735.594028	44.304999	63.913575
1734.805063	34.464341	63.918580
1734.293218	49.084676	63.923585
1733.939985	53.321175	63.928590
1733.305851	43.184695	63.933594
1732.310623	38.274643	63.938599
1731.578751	42.631197	63.943604
1731.060363	42.325648	63.948609
1730.381608	40.782473	63.953614
1728.731272	57.210990	63.958618
1728.154639	36.422889	63.963623
1727.785931	41.757788	63.968628
1727.537235	54.166521	63.973633
1726.926757	41.790244	63.978638
1726.152381	39.126891	63.983642
1725.917184	36.057794	63.988647
1724.991685	41.157859	63.993652
1724.391903	47.390446	63.998657
1723.979785	45.809655	64.003662
1723.267118	50.338199	64.008666
1722.948367	44.623719	64.013671
1721.429740	42.449142	64.018676
1720.547701	42.018431	64.023681
1720.149455	43.671235	64.028686
1719.503840	45.434286	64.033690
1719.281065	47.174334	64.038695
1717.935078	36.381398	64.043700
1716.988927	52.346425	64.048705
1716.328076	43.040490	64.053710
1715.968319	48.530083	64.058714
1716.023847	34.357602	64.063719
1715.484919	44.754572	64.068724
1714.879596	38.317662	64.073729
1714.157627	30.913720	64.078734
1712.582626	52.783186	64.083738
1712.418969	44.500536	64.088743
1711.626017	42.142902	64.093748
1710.864206	47.287935	64.098753
1710.936756	41.495541	64.103758
1709.208976	39.535534	64.108762
1708.511993	45.887636	64.113767
1707.938037	48.511334	64.118772
1707.906823	41.495978	64.123777
1707.591292	42.142200	64.128782
1706.885818	50.187665	64.133786
1705.867935	45.714867	64.138791
1705.019340	48.194535	64.143796
1704.122272	43.975353	64.148801
1703.585844	61.836978	64.153806
1702.980245	50.926445	64.158810
1702.710963	41.780665	64.163815
1701.706488	45.619149	64.168820
1700.979799	63.487342	64.173825
1700.710070	43.841057	64.178830
1699.772889	48.252305	64.183834
1699.504610	33.248195	64.188839
1698.136269	41.703282	64.193844
1697.733265	46.931673	64.198849
1697.090675	39.297513	64.203854
1696.063608	38.908769	64.208858
1695.635872	58.009913	64.213863
1695.388551	37.978469	64.218868
1694.856690	40.272218	64.223873
1694.319300	37.899229	64.228878
1693.519332	46.328697	64.233882
1692.939817	29.510133	64.238887
1691.288708	58.956079	64.243892
1690.744531	49.492850	64.248897
1690.102738	33.245551	64.253902
1689.295683	51.826638	64.258906
1689.496273	34.664972	64.263911
1688.847011	32.847476	64.268916
1688.200452	36.881416	64.273921
1688.079789	38.048601	64.278926
1686.760536	45.601798	64.283930
1686.243554	40.309884	64.288935
1685.328040	32.540893	64.293940
1684.100190	35.826677	64.298945
1683.441925	45.205008	64.303950
1682.484385	52.683410	64.308954
1682.669495	31.627692	64.313959
1681.743234	44.525647	64.318964
1681.532067	49.889143	64.323969
1681.349061	26.873473	64.328974
1680.694186	36.725906	64.333978
1679.556151	52.456499	64.338983
1679.034157	32.437159	64.343988
1678.060516	31.434408	64.348993
1677.165460	48.034695	64.353998
1676.144614	46.515911	64.359002
1675.689487	41.985278	64.364007
1675.301265	32.989285	64.369012
1674.453489	40.098600	64.374017
1674.250664	39.671978	64.379022
1673.796097	42.998938	64.384026
1673.195074	45.850861	64.389031
1672.055062	49.761345	64.394036
1671.228587	49.471631	64.399041
1670.913247	45.603167	64.404046
1670.226995	61.451238	64.409050
1669.280345	43.249699	64.414055
1668.630884	48.709622	64.419060
1667.677865	48.249205	64.424065
1667.926640	39.405907	64.429070
1666.756553	39.878802	64.434074
1666.410433	49.742124	64.439079
1665.764090	45.528860	64.444084
1664.851244	41.375277	64.449089
1664.441325	47.285988	64.454094
1663.631210	41.532881	64.459098
1662.856300	44.557502	64.464103
1662.024204	44.792214	64.469108
1661.388649	42.898432	64.474113
1661.256056	36.709712	64.479118
1660.008682	46.916459	64.484122
1659.345713	49.926454	64.489127
1658.381485	40.459004	64.494132
1658.187114	48.375983	64.499137
1657.818281	39.890979	64.504142
1657.095463	41.054472	64.509146
1656.829717	42.836041	64.514151
1655.539796	36.203556	64.519156
1654.874423	44.751995	64.524161
1654.701831	34.584810	64.529166
1653.481703	34.650936	64.534170
1652.490493	47.494565	64.539175
1652.184050	51.949135	64.544180
1651.077739	34.246049	64.549185
1651.296072	39.186514	64.554190
1650.595790	55.941949	64.559194
1650.422139	41.796413	64.564199
1648.927422	43.713284	64.569204
1648.054202	39.928714	64.574209
1647.773872	42.097364	64.579214
1647.029691	41.548589	64.584218
1646.150254	33.538926	64.589223
1645.474031	38.719259	64.594228
1644.796164	38.323949	64.599233
1644.684077	41.457741	64.604238
1643.986892	48.601491	64.609242
1643.569201	34.086315	64.614247
1642.364610	38.705631	64.619252
1641.914630	47.038515	64.624257
1641.089183	38.007907	64.629262
1639.740227	44.036251	64.634266
1639.228665	43.218722	64.639271
1639.096408	39.038917	64.644276
1638.514483	36.157370	64.649281
1638.365721	27.796685	64.654286
1637.531125	41.976295	64.659290
1636.528145	46.740202	64.664295
1635.936241	45.954359	64.669300
1635.044403	48.146038	64.674305
1634.440702	37.918033	64.679310
1633.754864	40.986857	64.684314
1632.792090	33.310548	64.689319
1632.083679	30.849629	64.694324
1631.659910	28.703025	64.699329
1631.369803	42.628989	64.704334
1630.830188	36.547507	64.709338
1630.235705	30.389592	64.714343
1628.951231	39.474758	64.719348
1628.158084	44.960667	64.724353
1627.953231	37.152918	64.729358
1627.520063	38.710359	64.734362
1626.737564	33.665639	64.739367
1625.757350	34.480537	64.744372
1625.078593	41.786934	64.749377
1624.837117	39.177724	64.754382
1623.858919	46.271505	64.759386
1623.053804	29.573962	64.764391
1622.433055	36.562070	64.769396
1621.924154	39.260601	64.774401
1621.590109	32.235020	64.779406
1620.722675	41.056828	64.784410
1620.044217	28.697708	64.789415
1619.320757	39.201267	64.794420
1618.790302	42.906129	64.799425
1618.362835	28.417749	64.804430
1617.263593	40.154216	64.809434
1616.371220	33.401831	64.814439
1615.821808	27.350297	64.819444
1615.412109	40.595116	64.824449
1615.417041	33.490455	64.829454
1614.059049	46.133749	64.834458
1613.673468	29.052605	64.839463
1613.084766	44.672285	64.844468
1611.687841	48.038579	64.849473
1611.319188	33.881463	64.854478
1610.607691	44.953962	64.859482
1610.466957	30.065230	64.864487
1609.238759	38.599011	64.869492
1608.170883	34.583618	64.874497
1607.723435	28.068049	64.879502
1607.133083	48.708830	64.884506
1606.784951	40.110166	64.889511
1606.259197	36.763981	64.894516
1605.851590	37.568339	64.899521
1605.100085	35.417037	64.904526
1603.941744	39.999062	64.909530
1603.898484	30.166144	64.914535
1603.021206	40.408725	64.919540
1602.028211	39.730764	64.924545
1601.401711	27.014905	64.929550
1600.529012	39.033918	64.934554
1600.411647	34.077496	64.939559
1599.360875	40.258751	64.944564
1598.167779	34.246406	64.949569
1598.102441	33.034731	64.954574
1597.452006	40.469092	64.959578
1597.216770	34.686181	64.964583
1596.770310	39.765369	64.969588
1595.548554	38.098772	64.974593
1595.339550	29.203634	64.979598
1594.184903	32.657594	64.984602
1593.306848	41.064794	64.989607
1592.513786	28.725471	64.994612
1592.072553	29.011643	64.999617
1591.942317	34.874769	65.004622
1591.139047	40.496330	65.009626
1590.512819	37.375838	65.014631
1589.379629	32.590267	65.019636
1588.794574	44.077904	65.024641
1588.685894	30.322603	65.029646
1587.459588	29.449912	65.034650
1586.800806	35.327627	65.039655
1585.984994	28.336019	65.044660
1585.587002	41.976357	65.049665
1585.498148	31.707577	65.054670
1584.295271	41.937240	65.059674
1583.263289	41.558783	65.064679
1582.539101	37.310607	65.069684
1582.360357	28.535239	65.074689
1582.102011	25.528186	65.079694
1581.370044	33.696141	65.084698
1580.421423	35.543633	65.089703
1579.631312	38.709456	65.094708
1579.111739	30.499152	65.099713
1578.821796	28.818556	65.104718
1577.202202	31.773980	65.109722
1576.857707	35.160730	65.114727
1576.693748	30.066640	65.119732
1576.011760	30.832597	65.124737
1574.690056	30.039722	65.129742
1573.873374	35.649224	65.134746
1573.688329	38.299462	65.139751
1573.352508	35.385139	65.144756
1572.652659	41.513803	65.149761
1571.827007	38.384001	65.154766
1570.941457	23.599429	65.159770
1570.419981	35.702986	65.164775
1570.325537	32.058057	65.169780
1568.875426	29.757575	65.174785
1568.370899	39.158800	65.179790
1567.632170	40.301191	65.184794
1567.297125	41.198101	65.189799
1566.802793	36.400920	65.194804
1565.437443	35.455717	65.199809
1564.940480	30.931759	65.204814
1564.220912	39.690663	65.209818
1563.856768	35.654938	65.214823
1563.621892	38.724664	65.219828
1562.256712	35.087676	65.224833
1561.695716	27.049534	65.229838
1560.869516	29.815833	65.234842
1560.475274	35.397641	65.239847
1560.192925	34.062758	65.244852
1559.436853	37.962742	65.249857
1558.876860	33.388877	65.254862
1557.740495	38.148770	65.259866
1557.273297	28.290181	65.264871
1557.011530	33.018340	65.269876
1555.577168	41.203292	65.274881
1554.899009	39.428268	65.279886
1554.329275	42.193244	65.284890
1554.025255	37.093024	65.289895
1553.722921	35.646204	65.294900
1552.339234	39.715294	65.299905
1551.974318	38.759369	65.304910
1551.150912	39.861605	65.309914
1550.872112	31.936315	65.314919
1550.226389	49.939867	65.319924
1549.367110	45.831432	65.324929
1548.923257	34.778575	65.329934
1548.073764	35.714651	65.334938
1547.309346	43.050443	65.339943
1546.390425	33.140630	65.344948
1545.733176	39.470679	65.349953
1545.639127	26.564589	65.354958
1544.760645	34.218110	65.359962
1544.089189	37.261015	65.364967
1543.405879	35.928343	65.369972
1542.878847	33.642050	65.374977
1542.316567	35.737240	65.379982
1540.984592	34.854554	65.384986
1540.442171	29.213500	65.389991
1540.463477	31.431996	65.394996
1539.637942	27.174711	65.400001
1539.002877	24.142369	65.405006
1537.653340	36.265543	65.410010
1537.259706	32.958304	65.415015
1536.804486	28.637448	65.420020
1536.335776	41.035391	65.425025
1535.897661	29.420256	65.430030
1534.641505	34.142423	65.435034
1533.950835	27.276026	65.440039
1533.422072	36.354686	65.445044
1532.766011	27.324023	65.450049
1531.823036	25.461780	65.455054
1531.177854	27.264226	65.460058
1530.671803	36.695656	65.465063
1530.564690	42.359574	65.470068
1529.637774	38.526814	65.475073
1529.027099	38.324277	65.480078
1528.282002	26.472507	65.485082
1527.895160	30.908316	65.490087
1526.752580	33.057871	65.495092
1525.797980	33.357822	65.500097
1525.321385	43.486293	65.505102
1524.787426	38.146659	65.510106
1524.526105	26.158097	65.515111
1524.013477	29.458031	65.520116
1522.925314	34.834728	65.525121
1522.307250	33.461734	65.530126
1521.583313	41.106477	65.535130
1520.928461	37.154798	65.540135
1520.255418	33.469353	65.545140
1519.418693	38.282569	65.550145
1518.972380	32.965280	65.555150
1518.657439	38.326342	65.560154
1517.997279	42.438170	65.565159
1517.258702	33.827459	65.570164
1516.320751	41.266522	65.575169
1515.217645	41.452884	65.580174
1513.949487	39.823662	65.585178
1513.981608	30.611112	65.590183
1513.794159	35.163468	65.595188
1513.064544	31.001331	65.600193
1512.916440	27.439049	65.605198
1511.945523	38.956466	65.610202
1511.214326	23.556061	65.615207
1510.665694	33.707012	65.620212
1509.743391	41.700234	65.625217
1508.856127	31.977790	65.630222
1508.372137	38.507387	65.635226
1507.705186	30.027221	65.640231
1507.209163	38.042586	65.645236
1506.451313	43.209114	65.650241
1505.654775	38.754848	65.655246
1505.012417	45.766913	65.660250
1504.687003	36.642713	65.665255
1503.757936	36.331510	65.670260
1502.755340	37.624655	65.675265
1502.334198	37.059281	65.680270
1501.646058	52.041942	65.685274
1501.560577	42.955302	65.690279
1500.533275	33.313459	65.695284
1499.641345	38.195376	65.700289
1499.268344	41.633972	65.705294
1498.536059	46.596174	65.710298
1498.113177	36.899281	65.715303
1497.249681	29.743405	65.720308
1496.619203	36.185898	65.725313
1496.006348	32.681699	65.730318
1494.676764	43.738899	65.735322
1494.304340	33.294428	65.740327
1493.979121	45.626999	65.745332
1493.118985	38.380703	65.750337
1493.015148	29.817364	65.755342
1491.797455	43.226854	65.760346
1491.109254	44.731808	65.765351
1490.403991	34.871642	65.770356
1489.948603	44.687676	65.775361
1489.405981	36.553594	65.780366
1488.514215	35.711364	65.785370
1487.793103	39.959035	65.790375
1487.149556	39.593004	65.795380
1486.758923	42.502990	65.800385
1485.865676	32.144442	65.805390
1484.877317	45.558491	65.810394
1484.416334	42.167349	65.815399
1484.010479	36.515643	65.820404
1483.490202	41.704344	65.825409
1482.797482	43.914889	65.830414
1482.248125	41.685770	65.835418
1481.710046	39.740278	65.840423
1480.648652	49.099129	65.845428
1479.671898	41.264265	65.850433
1479.090517	37.329307	65.855438
1478.456969	39.243454	65.860442
1478.241008	51.710049	65.865447
1477.347021	38.834893	65.870452
1476.399904	41.957890	65.875457
1476.159855	37.579196	65.880462
1475.359990	39.669580	65.885466
1475.011215	38.755255	65.890471
1474.361290	41.320110	65.895476
1473.629248	35.567285	65.900481
1473.024943	36.010275	65.905486
1471.578947	40.798909	65.910490
1470.953873	37.988915	65.915495
1470.770934	33.312576	65.920500
1470.403482	45.207174	65.925505
1470.077823	30.376245	65.930510
1468.834685	47.285761	65.935514
1468.028454	37.376996	65.940519
1467.721712	38.551684	65.945524
1466.521782	43.367446	65.950529
1466.025593	37.588179	65.955534
1465.193497	42.083720	65.960538
1465.001897	39.998017	65.965543
1464.472926	33.657857	65.970548
1463.063138	53.187855	65.975553
1462.736412	37.519759	65.980558
1462.249890	40.683098	65.985562
1461.975403	48.205967	65.990567
1461.117772	38.707480	65.995572
1460.183391	45.029553	66.000577
1459.777649	41.795211	66.005582
1458.471518	48.229980	66.010586
1457.569096	43.988093	66.015591
1456.913665	41.373730	66.020596
1456.260932	50.180383	66.025601
1456.416891	38.141280	66.030606
1455.972980	51.822040	66.035610
1455.485852	42.296210	66.040615
1454.843687	36.961176	66.045620
1453.748455	48.285491	66.050625
1453.421137	39.130065	66.055630
1452.039522	42.189664	66.060634
1451.245843	40.078227	66.065639
1450.894189	37.417166	66.070644
1450.128385	42.075634	66.075649
1449.602627	42.116653	66.080654
1448.621273	46.546039	66.085658
1448.092989	31.818277	66.090663
1448.037745	34.025284	66.095668
1446.782436	37.424342	66.100673
1446.354226	37.904005	66.105678
1445.645233	53.268441	66.110682
1445.045345	39.141812	66.115687
1444.783268	39.074697	66.120692
1443.634354	47.513947	66.125697
1443.056657	29.545642	66.130702
1442.589897	40.699111	66.135706
1441.909935	40.632181	66.140711
1440.835945	31.707391	66.145716
1440.027585	37.675137	66.150721
1439.990423	31.095978	66.155726
1439.058226	42.383343	66.160730
1437.977658	47.180148	66.165735
1437.706243	43.298434	66.170740
1437.022626	43.225779	66.175745
1437.060825	36.565257	66.180750
1435.729990	43.546411	66.185754
1434.944567	45.811124	66.190759
1434.640168	36.104880	66.195764
1433.924444	39.433955	66.200769
1433.051306	22.690558	66.205774
1432.152193	40.351191	66.210778
1431.631086	37.169883	66.215783
1431.562490	38.535375	66.220788
1430.599894	36.438177	66.225793
1429.673495	27.876277	66.230798
1428.960914	35.162852	66.235802
1428.539133	38.385289	66.240807
1428.147504	28.790683	66.245812
1426.950433	45.915230	66.250817
1426.946770	38.810370	66.255822
1426.269571	40.255245	66.260826
1424.880102	33.301260	66.265831
1424.433914	41.900050	66.270836
1423.520670	34.550266	66.275841
1423.368521	34.164494	66.280846
1422.703533	27.674086	66.285850
1421.898792	37.618181	66.290855
1421.384792	33.648878	66.295860
1420.875979	36.082509	66.300865
1420.033499	36.878746	66.305870
1418.785405	35.309459	66.310874
1418.257701	41.579520	66.315879
1417.946162	43.989684	66.320884
1417.444493	34.377874	66.325889
1416.653517	34.052640	66.330894
1415.629418	44.077336	66.335898
1415.209787	36.664868	66.340903
1414.852117	36.436337	66.345908
1414.014677	38.332445	66.350913
1413.461001	41.820267	66.355918
1412.484543	36.117349	66.360922
1411.838937	38.161156	66.365927
1411.447126	36.974571	66.370932
1410.513373	39.750125	66.375937
1410.284317	40.590786	66.380942
1409.226674	32.070253	66.385946
1408.840572	45.185176	66.390951
1408.261471	28.948538	66.395956
1406.778412	35.114990	66.400961
1406.705423	25.174867	66.405966
1406.183082	23.389313	66.410970
1405.765625	28.225799	66.415975
1404.708925	26.387989	66.420980
1403.778743	25.681200	66.425985
1403.514597	24.529517	66.430990
1402.202814	38.468053	66.435994
1401.638433	40.268726	66.440999
1401.016124	30.027997	66.446004
1400.478165	35.820314	66.451009
1400.303999	35.972610	66.456014
1400.078122	35.122337	66.461018
1399.051551	27.998730	66.466023
1398.232863	35.724784	66.471028
1397.539398	34.748568	66.476033
1396.922379	24.581118	66.481038
1396.194955	36.632270	66.486042
1395.383528	35.241160	66.491047
1395.053373	27.497524	66.496052
1393.804315	33.929551	66.501057
1392.944993	40.656010	66.506062
1392.503896	42.315669	66.511066
1391.878706	32.783424	66.516071
1391.931392	35.772759	66.521076
1391.545131	33.702236	66.526081
1390.701199	28.910209	66.531086
1389.788021	37.297810	66.536090
1388.648545	30.264690	66.541095
1387.979704	33.586323	66.546100
1387.389188	31.679149	66.551105
1387.330278	30.179467	66.556110
1386.024571	37.623405	66.561114
1385.073824	37.271539	66.566119
1384.676428	25.444984	66.571124
1384.049003	40.430609	66.576129
1384.186833	29.088234	66.581134
1383.126428	35.594353	66.586138
1382.424871	30.257747	66.591143
1381.881464	29.535216	66.596148
1380.667131	40.561524	66.601153
1380.262541	31.596591	66.606158
1379.604782	38.644237	66.611162
1378.876717	30.727319	66.616167
1378.804446	27.162457	66.621172
1377.465998	35.366933	66.626177
1376.879062	30.582944	66.631182
1376.629306	39.937381	66.636186
1375.861636	31.307697	66.641191
1374.786033	32.424844	66.646196
1373.983031	34.575676	66.651201
1373.587703	30.202760	66.656206
1373.583868	30.182908	66.661210
1372.545379	33.358307	66.666215
1371.742270	37.549655	66.671220
1370.781625	44.905639	66.676225
1370.590430	34.966959	66.681230
1369.413087	39.682979	66.686234
1368.438014	40.412002	66.691239
1368.156738	31.846924	66.696244
1367.578798	43.245145	66.701249
1367.572447	34.021376	66.706254
1366.679091	30.579148	66.711258
1365.606587	36.405980	66.716263
1365.304745	29.260222	66.721268
1364.580655	32.789331	66.726273
1363.412746	31.346093	66.731278
1362.876706	37.548102	66.736282
1362.236216	34.669629	66.741287
1361.945631	28.452448	66.746292
1361.122095	40.755421	66.751297
1360.843875	31.920210	66.756302
1359.845493	34.590941	66.761306
1359.432164	32.143119	66.766311
1358.664132	29.166655	66.771316
1357.348720	28.172628	66.776321
1357.166677	31.046316	66.781326
1356.504223	35.456573	66.786330
1355.892796	36.309137	66.791335
1355.191689	29.261541	66.796340
1354.371774	32.419547	66.801345
1354.451780	31.178469	66.806350
1353.117323	38.029351	66.811354
1352.124433	26.265929	66.816359
1351.531789	32.773391	66.821364
1350.960506	38.526861	66.826369
1351.123222	26.616007	66.831374
1350.183910	40.908499	66.836378
1349.301903	35.934887	66.841383
1348.864322	36.815009	66.846388
1348.002075	43.437871	66.851393
1346.849561	25.696601	66.856398
1346.313225	33.063980	66.861402
1345.583757	33.738199	66.866407
1345.446023	32.711501	66.871412
1344.954529	38.453864	66.876417
1344.217497	28.909456	66.881422
1343.291922	29.275820	66.886426
1342.648543	33.391322	66.891431
1341.844582	26.741690	66.896436
1341.236512	36.859533	66.901441
1340.834438	27.359648	66.906446
1340.388343	31.885317	66.911450
1339.391416	31.955531	66.916455
1338.741667	32.115628	66.921460
1338.206729	29.357573	66.926465
1337.614275	38.145193	66.931470
1336.516562	28.598205	66.936474
1335.846217	36.437881	66.941479
1335.612812	28.563764	66.946484
1334.601812	23.982815	66.951489
1333.865350	37.207043	66.956494
1333.167262	33.191335	66.961498
1332.850399	27.225910	66.966503
1332.442031	26.679034	66.971508
1331.120447	27.360659	66.976513
1330.818176	30.895255	66.981518
1329.964687	25.655357	66.986522
1329.679372	22.091253	66.991527
1328.676656	25.473860	66.996532
1327.805857	30.371387	67.001537
1327.445164	30.110235	67.006542
1326.774200	28.420862	67.011546
1326.369399	31.172275	67.016551
1325.748884	37.321489	67.021556
1324.642472	39.238308	67.026561
1324.108069	28.936325	67.031566
1323.515455	43.016020	67.036570
1322.500122	32.121890	67.041575
1322.214114	25.295311	67.046580
1321.402953	40.888869	67.051585
1321.139536	37.012211	67.056590
1319.862886	35.452244	67.061594
1319.366816	37.732487	67.066599
1318.962173	32.842264	67.071604
1318.336561	34.372001	67.076609
1317.985778	27.806445	67.081614
1316.791319	45.503017	67.086618
1316.416766	28.491183	67.091623
1315.852904	26.936168	67.096628
1314.435284	32.105129	67.101633
1313.812379	30.803918	67.106638
1313.644224	32.549500	67.111642
1313.253392	33.400119	67.116647
1312.585731	32.386710	67.121652
1311.209797	24.629587	67.126657
1310.927886	25.261047	67.131662
1310.280251	30.476324	67.136666
1310.035578	20.536705	67.141671
1308.837732	26.120140	67.146676
1308.004866	39.403853	67.151681
1307.875906	30.097087	67.156686
1306.926053	26.108801	67.161690
1305.981208	32.508268	67.166695
1305.645751	30.648871	67.171700
1305.247376	30.573478	67.176705
1304.743204	21.045685	67.181710
1303.592957	27.063084	67.186714
1303.027517	25.502015	67.191719
1302.438037	23.817041	67.196724
1301.472799	33.283647	67.201729
1300.918360	22.500757	67.206734
1300.170660	21.425964	67.211738
1299.775965	35.622414	67.216743
1299.495904	27.290539	67.221748
1297.919051	31.133430	67.226753
1297.767867	23.299865	67.231758
1297.069604	28.501116	67.236762
1296.657115	30.641922	67.241767
1295.953244	36.914776	67.246772
1295.020939	38.676198	67.251777
1294.670526	31.020955	67.256782
1293.930518	25.159081	67.261786
1293.123272	27.635450	67.266791
1292.687396	26.823306	67.271796
1291.827339	34.992760	67.276801
1290.821565	20.503404	67.281806
1290.084190	21.212010	67.286810
1289.350606	19.281880	67.291815
1289.432449	26.970431	67.296820
1288.694752	18.886357	67.301825
1288.268648	26.209407	67.306830
1287.118875	26.141523	67.311834
1286.463748	21.196522	67.316839
1286.229666	27.486142	67.321844
1284.753617	30.586067	67.326849
1284.552927	29.646649	67.331854
1284.052969	31.195838	67.336858
1283.265563	38.388688	67.341863
1282.348797	32.222195	67.346868
1281.223943	39.071321	67.351873
1281.414720	36.555849	67.356878
1281.133434	33.235527	67.361882
1279.868983	39.769395	67.366887
1279.495430	23.257294	67.371892
1278.741038	33.737438	67.376897
1278.083528	29.366804	67.381902
1277.090980	26.580600	67.386906
1276.479441	20.083322	67.391911
1276.046230	22.126503	67.396916
1274.791984	43.000559	67.401921
1274.028087	20.227196	67.406926
1273.915719	26.092203	67.411930
1273.421805	29.690388	67.416935
1272.953307	22.654724	67.421940
1272.106035	32.697069	67.426945
1271.198851	20.797070	67.431950
1270.708378	30.344308	67.436954
1270.056290	29.585468	67.441959
1269.502417	29.288810	67.446964
1268.470394	33.141282	67.451969
1268.249161	24.964058	67.456974
1267.687336	34.867983	67.461978
1266.596188	34.183684	67.466983
1265.974806	35.238117	67.471988
1265.239152	26.729540	67.476993
1264.911743	14.065611	67.481998
1263.718163	32.359683	67.487002
1263.093359	31.806232	67.492007
1262.657692	38.872201	67.497012
1262.043445	42.150493	67.502017
1262.227011	28.224216	67.507022
1260.899243	34.960538	67.512026
1260.122266	27.789427	67.517031
1259.649174	38.931297	67.522036
1258.452287	40.007854	67.527041
1258.112965	27.459346	67.532046
1257.222311	31.529030	67.537050
1257.020457	44.800731	67.542055
1256.161345	32.055757	67.547060
1255.240077	33.604134	67.552065
1254.918470	26.431581	67.557070
1254.384815	22.222606	67.562074
1253.538133	34.021515	67.567079
1253.024230	35.192897	67.572084
1252.295791	40.011045	67.577089
1251.833447	24.380360	67.582094
1250.492603	34.977411	67.587098
1249.951958	32.097286	67.592103
1249.768016	38.061984	67.597108
1248.706958	42.163500	67.602113
1248.166008	21.795725	67.607118
1247.648520	24.714869	67.612122
1247.003664	32.361278	67.617127
1246.463518	25.649236	67.622132
1245.732204	26.205510	67.627137
1245.243840	22.167524	67.632142
1244.216819	27.386369	67.637146
1243.092726	27.979869	67.642151
1242.944246	31.005912	67.647156
1242.152706	31.813028	67.652161
1241.954689	26.298636	67.657166
1240.854924	24.737392	67.662170
1239.792367	30.594223	67.667175
1239.530863	17.246487	67.672180
1239.021902	26.490750	67.677185
1238.510684	19.343623	67.682190
1237.352553	28.853530	67.687194
1236.665192	10.566897	67.692199
1236.295927	28.610054	67.697204
1236.099514	23.775047	67.702209
1235.090433	11.203753	67.707214
1234.177079	35.032302	67.712218
1233.696011	30.527974	67.717223
1233.430352	21.635608	67.722228
1232.297047	38.177650	67.727233
1231.618298	20.504624	67.732238
1230.720708	18.624243	67.737242
1230.541497	24.271229	67.742247
1229.635592	20.758515	67.747252
1228.869848	24.081399	67.752257
1228.221170	20.933044	67.757262
1227.948447	27.094773	67.762266
1227.290811	31.333986	67.767271
1226.324688	20.026830	67.772276
1225.738089	28.096044	67.777281
1225.551331	24.754394	67.782286
1224.112192	18.734072	67.787290
1223.582081	22.341172	67.792295
1223.420123	19.195844	67.797300
1222.386204	35.113403	67.802305
1221.483789	31.347832	67.807310
1220.903639	34.631747	67.812314
1220.372139	30.455550	67.817319
1220.327229	25.189616	67.822324
1219.140541	30.525320	67.827329
1218.459191	16.274567	67.832334
1217.822867	31.630603	67.837338
1217.057921	33.844812	67.842343
1216.359644	15.537842	67.847348
1215.458216	11.575011	67.852353
1214.857138	16.888550	67.857358
1214.388354	27.307514	67.862362
1213.966561	29.061896	67.867367
1213.864407	19.522241	67.872372
1212.684166	21.985408	67.877377
1212.367047	14.974575	67.882382
1211.096988	25.390076	67.887386
1210.305399	23.453424	67.892391
1210.118606	17.099928	67.897396
1209.492752	24.079448	67.902401
1208.438501	18.338539	67.907406
1207.645631	17.127461	67.912410
1207.039433	20.962696	67.917415
1206.937396	17.445157	67.922420
1205.897262	26.250365	67.927425
1205.224354	13.548358	67.932430
1204.523804	26.637579	67.937434
1203.852836	24.624980	67.942439
1203.761248	25.090573	67.947444
1202.707127	17.361191	67.952449
1202.267578	16.976985	67.957454
1201.081343	27.432775	67.962458
1200.041278	17.009412	67.967463
1199.698481	29.759482	67.972468
1198.747210	19.769834	67.977473
1198.853031	21.374084	67.982478
1198.350900	28.543659	67.987482
1197.572075	30.903578	67.992487
1196.900113	24.877959	67.997492
1195.947759	30.794548	68.002497
1195.772454	21.304372	68.007502
1194.739765	18.956654	68.012506
1193.963891	26.780017	68.017511
1193.824837	27.366695	68.022516
1192.539329	24.925147	68.027521
1191.653538	19.792940	68.032526
1190.982741	14.522472	68.037530
1190.733845	21.834692	68.042535
1190.303255	15.362281	68.047540
1189.485610	20.278199	68.052545
1188.789663	24.655969	68.057550
1188.368331	17.164993	68.062554
1187.538777	17.240187	68.067559
1186.560392	16.271497	68.072564
1185.770531	13.788978	68.077569
1185.571716	13.942054	68.082574
1185.138287	20.462063	68.087578
1183.991754	19.887529	68.092583
1183.353532	10.504095	68.097588
1182.837017	24.697831	68.102593
1182.649707	22.900046	68.107598
1181.404456	15.948515	68.112602
1180.342575	18.381835	68.117607
1180.356698	22.727104	68.122612
1179.914789	24.170889	68.127617
1179.015176	17.203813	68.132622
1178.062065	26.931860	68.137626
1177.572704	25.388684	68.142631
1176.655533	19.052002	68.147636
1175.454504	28.119340	68.152641
1175.137706	20.755238	68.157646
1174.989554	25.250889	68.162650
1174.269187	26.508733	68.167655
1174.364628	10.388855	68.172660
1173.084014	28.042379	68.177665
1172.891625	19.106836	68.182670
1171.461332	12.282508	68.187674
1170.581603	19.215679	68.192679
1170.403383	12.955440	68.197684
1169.607372	17.456354	68.202689
1169.141087	23.700905	68.207694
1168.259321	31.886455	68.212698
1167.729609	21.599551	68.217703
1167.516487	22.426658	68.222708
1165.902736	27.525963	68.227713
1165.446791	23.694142	68.232718
1165.005641	16.013944	68.237722
1164.392435	28.895325	68.242727
1163.392722	22.740501	68.247732
1162.478546	22.531130	68.252737
1162.218566	16.387968	68.257742
1161.833056	22.204952	68.262746
1161.288924	12.142692	68.267751
1160.614397	18.939156	68.272756
1159.455069	26.303137	68.277761
1159.205699	20.803234	68.282766
1158.559086	31.116451	68.287770
1157.605016	32.610157	68.292775
1156.902740	23.304717	68.297780
1156.165091	37.276603	68.302785
1156.155772	28.247290	68.307790
1155.056257	26.730197	68.312794
1154.179860	30.012356	68.317799
1153.962892	26.178798	68.322804
1153.220344	34.600821	68.327809
1152.294568	28.554084	68.332814
1152.034328	25.310857	68.337818
1151.103939	31.835798	68.342823
1150.591906	25.185542	68.347828
1148.978797	32.708431	68.352833
1148.733498	29.114335	68.357838
1148.513835	35.565664	68.362842
1148.183560	28.295167	68.367847
1148.021165	30.900820	68.372852
1146.770338	34.113228	68.377857
1145.744405	31.991527	68.382862
1144.782325	22.859871	68.387866
1143.880687	23.025388	68.392871
1143.634824	30.818082	68.397876
1142.988846	31.617845	68.402881
1142.786271	22.710732	68.407886
1142.399749	25.192766	68.412890
1141.369744	22.483537	68.417895
1141.122757	25.798051	68.422900
1139.526760	34.789460	68.427905
1138.637617	21.024352	68.432910
1137.994398	29.436884	68.437914
1137.758178	25.729388	68.442919
1137.522950	28.564236	68.447924
1137.178476	38.517183	68.452929
1136.167674	21.622381	68.457934
1135.308560	39.119008	68.462938
1134.572720	33.199757	68.467943
1133.657667	29.660150	68.472948
1132.958156	32.441115	68.477953
1132.402547	15.812955	68.482958
1131.979991	42.616314	68.487962
1131.656641	28.628754	68.492967
1130.849020	23.217644	68.497972
1129.880122	29.526374	68.502977
1129.677023	22.681915	68.507982
1128.473042	29.417527	68.512986
1127.635729	37.466715	68.517991
1127.591459	28.187508	68.522996
1126.984234	34.113878	68.528001
1126.238402	21.127041	68.533006
1125.398363	19.715342	68.538010
1124.668885	22.180967	68.543015
1124.430363	31.276577	68.548020
1122.987924	33.726299	68.553025
1122.489341	29.749886	68.558030
1122.172011	17.812911	68.563034
1121.421534	30.465406	68.568039
1120.842779	24.849170	68.573044
1120.052435	29.241971	68.578049
1119.922059	18.648728	68.583054
1118.623834	24.153593	68.588058
1117.854358	16.746393	68.593063
1117.727909	26.809729	68.598068
1116.875369	27.714890	68.603073
1115.671397	22.232793	68.608078
1115.253101	34.614846	68.613082
1114.318726	37.657092	68.618087
1114.160175	28.930628	68.623092
1113.817796	38.891128	68.628097
1113.108214	28.624962	68.633102
1111.841364	33.090405	68.638106
1111.326757	33.657978	68.643111
1111.051856	32.331427	68.648116
1110.023183	40.953508	68.653121
1109.450800	33.180654	68.658126
1108.677714	30.701796	68.663130
1108.344309	37.603286	68.668135
1107.566837	32.499609	68.673140
1106.261627	37.630296	68.678145
1105.754486	37.433469	68.683150
1105.639460	26.494019	68.688154
1105.108667	33.682359	68.693159
1104.934511	21.396197	68.698164
1103.518202	34.055262	68.703169
1103.298737	31.034203	68.708174
1102.447606	30.559369	68.713178
1100.950126	30.149501	68.718183
1101.090997	31.114263	68.723188
1100.447055	47.072329	68.728193
1099.247109	36.330675	68.733198
1098.677899	34.335033	68.738202
1098.049034	37.983097	68.743207
1097.859902	20.564976	68.748212
1097.104123	33.409123	68.753217
1096.396598	34.387415	68.758222
1095.747065	31.631876	68.763226
1095.076711	38.777766	68.768231
1094.227193	31.607218	68.773236
1093.148829	38.387520	68.778241
1092.643072	27.508647	68.783246
1092.355515	30.569432	68.788250
1092.220874	33.902348	68.793255
1091.540653	30.044719	68.798260
1090.425893	36.950653	68.803265
1089.707009	31.687860	68.808270
1088.507021	26.719207	68.813274
1087.799000	33.464251	68.818279
1087.646233	31.485945	68.823284
1086.860086	35.376639	68.828289
1087.022402	40.939345	68.833294
1085.884168	25.324771	68.838298
1084.837488	33.063510	68.843303
1084.933500	27.128647	68.848308
1083.902473	32.190498	68.853313
1083.072483	23.370583	68.858318
1082.685263	24.690571	68.863322
1082.174256	23.062552	68.868327
1081.301307	23.682401	68.873332
1080.354479	30.481202	68.878337
1080.266297	27.765678	68.883342
1079.009236	27.754377	68.888346
1078.034887	28.652120	68.893351
1078.090206	25.607854	68.898356
1077.355833	24.737581	68.903361
1076.168353	34.381522	68.908366
1075.401392	38.371665	68.913370
1074.746951	33.308351	68.918375
1074.661297	28.624472	68.923380
1073.840574	30.588984	68.928385
1073.153760	28.200490	68.933390
1072.679464	40.274503	68.938394
1072.176948	16.560854	68.943399
1071.205170	37.757436	68.948404
1070.249192	35.641984	68.953409
1070.014989	25.965662	68.958414
1069.344715	37.511055	68.963418
1068.461167	32.667107	68.968423
1067.655736	22.649590	68.973428
1066.884771	37.107737	68.978433
1066.596175	26.363056	68.983438
1066.126113	30.200319	68.988442
1065.416798	24.239031	68.993447
1064.591313	19.896763	68.998452
1063.942653	27.181123	69.003457
1063.943739	33.942674	69.008462
1062.714788	21.871620	69.013466
1061.938268	29.945841	69.018471
1061.321720	21.371091	69.023476
1060.182405	33.695964	69.028481
1059.459348	23.865610	69.033486
1059.155324	19.205435	69.038490
1058.699213	32.864473	69.043495
1058.313364	24.790741	69.048500
1057.353540	35.442371	69.053505
1056.900477	25.939635	69.058510
1056.248825	26.680400	69.063514
1054.747536	26.625964	69.068519
1054.143718	9.325874	69.073524
1053.663824	41.111832	69.078529
1053.574870	19.185239	69.083534
1053.213825	16.839542	69.088538
1052.225879	27.486180	69.093543
1051.692730	29.278800	69.098548
1050.551245	25.224916	69.103553
1050.406087	30.331924	69.108558
1049.279663	30.064899	69.113562
1048.272343	33.006811	69.118567
1048.421270	30.340298	69.123572
1047.260419	36.499829	69.128577
1046.572214	31.476587	69.133582
1046.292307	21.238289	69.138586
1045.599437	32.564934	69.143591
1045.273281	18.819118	69.148596
1044.041579	31.578142	69.153601
1043.514477	29.205248	69.158606
1042.760940	38.485292	69.163610
1041.993078	35.466330	69.168615
1041.492115	29.982813	69.173620
1040.854957	36.081110	69.178625
1040.416939	24.890294	69.183630
1039.398378	27.649502	69.188634
1038.463692	28.238188	69.193639
1038.283069	22.177034	69.198644
1037.781525	26.249533	69.203649
1036.772636	29.842952	69.208654
1036.143352	22.807699	69.213658
1035.242318	26.853871	69.218663
1035.085182	24.165090	69.223668
1033.974005	39.940453	69.228673
1033.366909	28.368122	69.233678
1032.816841	24.374694	69.238682
1032.054194	35.179457	69.243687
1032.034864	25.882103	69.248692
1030.746262	29.199916	69.253697
1030.032349	19.355507	69.258702
1029.859960	21.238964	69.263706
1029.149578	28.928947	69.268711
1028.388114	29.934760	69.273716
1027.497281	32.205318	69.278721
1027.065374	26.042221	69.283726
1025.984416	26.425534	69.288730
1025.377689	25.476624	69.293735
1025.082624	21.578241	69.298740
1024.671826	26.103063	69.303745
1024.104341	13.929960	69.308750
1023.282248	20.286324	69.313754
1022.302089	29.351695	69.318759
1021.156634	21.794621	69.323764
1020.615503	27.828758	69.328769
1020.045401	25.210409	69.333774
1019.857667	24.396682	69.338778
1019.482643	35.948721	69.343783
1018.695027	32.765761	69.348788
1017.853129	32.702631	69.353793
1016.996710	29.920108	69.358798
1016.018322	30.807479	69.363802
1015.291469	28.322875	69.368807
1015.047778	21.423394	69.373812
1014.356737	30.836992	69.378817
1014.255378	27.751424	69.383822
1013.065216	23.741572	69.388826
1011.940305	27.831254	69.393831
1011.848301	26.647498	69.398836
1011.072347	18.845572	69.403841
1010.650067	25.994579	69.408846
1009.803196	35.396705	69.413850
1009.157697	27.774283	69.418855
1008.740165	22.175007	69.423860
1007.552319	28.327806	69.428865
1007.146695	17.675878	69.433870
1006.488441	34.962373	69.438874
1005.938988	37.620153	69.443879
1005.148052	20.423955	69.448884
1004.196840	25.391135	69.453889
1003.694232	28.793634	69.458894
1003.292342	37.227718	69.463898
1002.109499	34.017762	69.468903
1001.869425	22.912156	69.473908
1001.155832	30.123283	69.478913
1000.728853	25.892669	69.483918
1000.375125	19.474302	69.488922
999.363423	32.075343	69.493927
999.158008	22.858061	69.498932
997.669818	29.872323	69.503937
997.007255	23.466824	69.508942
996.821864	27.186267	69.513946
995.835535	30.435505	69.518951
995.180843	20.772489	69.523956
994.196297	34.935058	69.528961
994.024767	28.785731	69.533966
993.528483	18.335880	69.538970
992.175951	26.350379	69.543975
991.810904	19.191103	69.548980
991.110178	32.947407	69.553985
990.916584	19.437546	69.558990
990.364987	23.585822	69.563994
988.807852	33.220802	69.568999
988.962322	17.731765	69.574004
988.248488	27.264104	69.579009
987.087218	21.235988	69.584014
986.406771	17.283817	69.589018
986.001064	22.924266	69.594023
985.687094	23.076757	69.599028
984.355831	29.269731	69.604033
984.012666	18.037038	69.609038
983.669773	22.462754	69.614042
982.606163	27.987120	69.619047
982.131118	18.178838	69.624052
981.188891	19.046276	69.629057
980.673408	22.305752	69.634062
980.319130	19.889607	69.639066
979.412144	33.513159	69.644071
978.574855	16.945646	69.649076
977.905714	26.830405	69.654081
977.904342	18.151497	69.659086
976.845051	27.705689	69.664090
975.855753	19.603423	69.669095
975.187337	11.721328	69.674100
974.856784	32.711816	69.679105
974.027218	26.736577	69.684110
973.450635	25.582620	69.689114
972.604183	32.225140	69.694119
972.536659	16.859733	69.699124
971.226040	30.284167	69.704129
970.702446	27.350938	69.709134
969.976981	23.131556	69.714138
969.837138	25.875547	69.719143
969.254700	28.057630	69.724148
968.294197	19.671677	69.729153
967.743056	23.884536	69.734158
966.599611	23.869404	69.739162
965.573503	25.920242	69.744167
965.438799	23.357203	69.749172
964.793974	26.777606	69.754177
964.218802	19.219705	69.759182
963.572533	29.780465	69.764186
962.477329	24.085609	69.769191
962.563146	15.550519	69.774196
961.663687	27.834098	69.779201
961.109148	30.439080	69.784206
960.531455	24.251890	69.789210
959.562575	18.145871	69.794215
959.133546	28.345649	69.799220
957.905357	29.540860	69.804225
957.405084	19.776021	69.809230
957.037257	28.712439	69.814234
956.279572	25.840116	69.819239
955.748178	27.395942	69.824244
954.753817	24.108714	69.829249
954.452709	16.625474	69.834254
953.854488	22.429016	69.839258
952.825394	26.060371	69.844263
952.426014	20.412490	69.849268
951.564011	35.366087	69.854273
951.167549	26.537165	69.859278
950.317742	26.114210	69.864282
949.541876	26.130478	69.869287
949.452334	18.809107	69.874292
948.163309	29.513144	69.879297
947.231091	29.164802	69.884302
946.925525	29.697567	69.889306
946.411589	35.752620	69.894311
946.155537	29.853282	69.899316
944.720774	40.828090	69.904321
943.898806	29.799316	69.909326
943.911161	31.219738	69.914330
943.299495	32.748918	69.919335
942.363478	23.379834	69.924340
941.687236	21.428071	69.929345
941.344145	23.843297	69.934350
940.449107	24.696934	69.939354
939.478700	30.390980	69.944359
938.876098	18.835322	69.949364
938.389396	23.216120	69.954369
938.027193	14.440101	69.959374
937.076328	28.859080	69.964378
936.498308	25.795755	69.969383
936.139401	23.154859	69.974388
935.012596	26.133171	69.979393
934.173583	15.070857	69.984398
933.859242	19.056813	69.989402
933.308065	33.420080	69.994407
932.885323	19.390057	69.999412
931.845936	18.469020	70.004417
931.328855	24.433113	70.009422
930.548242	26.244634	70.014426
929.270745	30.872695	70.019431
928.845907	20.036195	70.024436
928.052616	24.397977	70.029441
927.945100	15.296016	70.034446
927.558740	28.336854	70.039450
926.905017	26.357858	70.044455
925.805588	17.011636	70.049460
925.389116	33.674637	70.054465
924.720364	24.209417	70.059470
923.795572	22.122177	70.064474
922.803799	20.212747	70.069479
922.701394	24.995997	70.074484
921.917222	33.509840	70.079489
921.072631	26.079974	70.084494
920.490185	21.795274	70.089498
919.869282	22.652600	70.094503
919.728219	15.585426	70.099508
918.782544	25.421163	70.104513
917.824588	22.985982	70.109518
917.487377	16.583929	70.114522
916.612499	24.196034	70.119527
915.897810	17.680594	70.124532
915.317310	24.072654	70.129537
915.073247	24.808514	70.134542
914.354520	20.717383	70.139546
913.183359	23.841528	70.144551
912.811891	22.412104	70.149556
912.082011	20.410541	70.154561
911.106545	26.045478	70.159566
910.490452	30.800095	70.164570
909.417800	20.620178	70.169575
909.516239	25.037166	70.174580
909.153265	28.050046	70.179585
908.583412	18.353063	70.184590
907.639097	16.361974	70.189594
906.192037	28.669636	70.194599
905.632948	31.097164	70.199604
904.922266	27.246018	70.204609
904.774336	26.900608	70.209614
904.602414	24.609989	70.214618
903.399470	38.953989	70.219623
902.575018	27.129304	70.224628
901.919716	33.285704	70.229633
901.367398	29.187016	70.234638
901.102973	27.458296	70.239642
900.130343	27.679350	70.244647
899.634100	22.636649	70.249652
898.830181	29.152575	70.254657
898.184444	25.784660	70.259662
897.228960	21.061038	70.264666
896.434216	24.814383	70.269671
896.481690	19.961109	70.274676
896.023749	29.791772	70.279681
895.101946	23.471716	70.284686
894.804535	23.561661	70.289690
893.482695	20.529995	70.294695
892.607606	22.518981	70.299700
891.765709	23.638555	70.304705
891.819703	22.493069	70.309710
891.199953	20.567022	70.314714
889.821192	30.949489	70.319719
889.320368	23.023401	70.324724
888.775159	19.349346	70.329729
888.255733	19.849923	70.334734
887.816936	18.008614	70.339738
886.479988	25.618576	70.344743
886.263382	8.302665	70.349748
885.794963	20.471926	70.354753
884.838550	18.523770	70.359758
884.206866	16.200674	70.364762
883.238898	20.659649	70.369767
883.295829	24.939745	70.374772
882.890110	24.886087	70.379777
881.657340	22.950376	70.384782
881.140554	18.256287	70.389786
880.087326	24.703088	70.394791
879.330389	18.263767	70.399796
878.827772	30.405365	70.404801
878.209447	23.940828	70.409806
878.294769	18.551699	70.414810
877.135646	29.846921	70.419815
876.795127	29.847540	70.424820
875.825144	33.734433	70.429825
874.755051	25.036394	70.434830
874.129471	18.476825	70.439834
873.351332	42.976152	70.444839
873.454602	32.621710	70.449844
872.700986	26.147168	70.454849
871.552384	17.866888	70.459854
870.742514	31.180127	70.464858
870.053217	38.436302	70.469863
869.936137	22.284048	70.474868
869.260369	30.044244	70.479873
868.389758	18.075549	70.484878
868.109139	19.984123	70.489882
867.157818	24.096694	70.494887
866.322029	29.786684	70.499892
865.171307	28.508097	70.504897
865.202451	23.679498	70.509902
864.992386	18.739487	70.514906
863.819134	31.851953	70.519911
863.041048	30.424177	70.524916
862.799192	37.839365	70.529921
861.705760	30.080136	70.534926
860.953926	29.651079	70.539930
859.937957	29.282985	70.544935
860.008652	23.809454	70.549940
859.707430	26.083991	70.554945
858.579638	28.433316	70.559950
858.072695	25.014939	70.564954
857.174658	31.246248	70.569959
856.233383	32.602414	70.574964
855.166475	37.840361	70.579969
854.616282	28.343679	70.584974
854.356304	26.190077	70.589978
854.220961	29.087888	70.594983
853.914763	24.101679	70.599988
852.722836	32.311445	70.604993
852.002622	27.271287	70.609998
851.690696	18.622897	70.615002
850.262739	36.232176	70.620007
849.873347	22.703047	70.625012
849.378485	24.494342	70.630017
848.573007	26.412343	70.635022
847.777418	24.468564	70.640026
846.919673	24.089484	70.645031
846.905710	12.271449	70.650036
846.300538	28.086155	70.655041
845.652026	18.190411	70.660046
844.540313	16.112455	70.665050
843.958397	22.640363	70.670055
843.250965	23.002147	70.675060
842.160172	34.948799	70.680065
841.906181	24.994988	70.685070
841.317968	22.557756	70.690074
840.844588	28.891781	70.695079
840.261354	22.621936	70.700084
839.109782	24.202382	70.705089
838.546484	19.843698	70.710094
838.424808	23.048402	70.715098
836.869756	28.457085	70.720103
836.693483	20.540854	70.725108
835.902441	21.691773	70.730113
835.769224	18.926668	70.735118
835.430804	28.251054	70.740122
834.467572	27.297438	70.745127
833.659267	29.928643	70.750132
832.567115	32.937751	70.755137
831.954763	30.092796	70.760142
831.956330	31.790887	70.765146
830.488853	31.800586	70.770151
829.836220	20.856876	70.775156
829.103561	21.276292	70.780161
828.774929	23.205127	70.785166
828.701307	31.402474	70.790170
827.290709	25.543431	70.795175
826.803506	31.906466	70.800180
826.016866	35.119250	70.805185
825.693758	31.157554	70.810190
825.024531	20.697436	70.815194
824.225150	30.883636	70.820199
823.957165	23.664794	70.825204
822.620916	27.464930	70.830209
821.805063	28.058433	70.835214
821.518522	25.503805	70.840218
820.947846	26.263277	70.845223
820.572524	29.822156	70.850228
819.521499	25.001816	70.855233
819.048477	29.675332	70.860238
818.537022	25.910769	70.865242
817.126871	28.178905	70.870247
816.728546	25.864411	70.875252
815.991721	27.765186	70.880257
815.547746	29.188858	70.885262
815.419320	20.429268	70.890266
814.112823	29.896712	70.895271
813.928180	21.128725	70.900276
813.305083	24.816925	70.905281
811.961109	29.368892	70.910286
811.228602	22.298107	70.915290
810.666749	28.272498	70.920295
810.397968	24.772070	70.925300
810.050215	26.111044	70.930305
809.020641	19.776644	70.935310
808.340439	21.133845	70.940314
807.403491	38.671292	70.945319
807.012268	20.703549	70.950324
806.110499	24.458185	70.955329
805.543130	24.007667	70.960334
805.270997	19.429189	70.965338
804.370560	28.590737	70.970343
803.513547	17.644881	70.975348
802.712963	22.438344	70.980353
802.106859	21.443662	70.985358
802.039361	22.851561	70.990362
801.142796	29.882129	70.995367
800.145649	17.727038	71.000372
799.947632	34.191268	71.005377
799.223136	23.722610	71.010382
798.498391	24.747875	71.015386
797.497310	18.583979	71.020391
796.979037	31.447133	71.025396
796.723211	15.764823	71.030401
795.647074	22.117532	71.035406
795.114386	17.329808	71.040410
794.526497	31.993802	71.045415
794.127178	15.239980	71.050420
793.039010	26.274785	71.055425
792.634175	28.994734	71.060430
791.958288	15.298357	71.065434
790.825088	31.633920	71.070439
790.600935	13.653788	71.075444
790.139229	32.194164	71.080449
789.229509	22.245406	71.085454
788.165655	22.421102	71.090458
787.287758	27.228455	71.095463
787.028059	34.723750	71.100468
786.771401	17.863643	71.105473
786.295953	25.150437	71.110478
785.429607	24.818477	71.115482
784.578077	21.795578	71.120487
784.215450	27.255734	71.125492
782.808264	23.105514	71.130497
782.218135	25.197402	71.135502
782.001590	21.633472	71.140506
781.343403	24.400060	71.145511
780.445603	23.636313	71.150516
779.511035	23.047145	71.155521
779.314317	21.539465	71.160526
778.968173	20.561750	71.165530
777.952830	20.182552	71.170535
777.262607	20.913758	71.175540
776.549469	30.450756	71.180545
776.270495	20.280176	71.185550
775.649168	25.251683	71.190554
774.619997	27.347235	71.195559
774.346741	25.799702	71.200564
772.952111	27.466176	71.205569
772.093464	15.598122	71.210574
771.636402	18.555033	71.215578
771.286793	12.984424	71.220583
771.133636	23.249096	71.225588
769.983389	28.651719	71.230593
769.013499	22.449756	71.235598
768.627725	18.613161	71.240602
768.109837	31.058382	71.245607
767.837234	16.198728	71.250612
766.665921	17.771310	71.255617
766.005953	31.989486	71.260622
765.661661	20.853218	71.265626
764.617634	24.592670	71.270631
763.938372	35.970807	71.275636
763.358213	31.720475	71.280641
762.828758	16.058082	71.285646
762.147843	22.551303	71.290650
761.022511	28.577561	71.295655
760.670502	19.279590	71.300660
760.305117	22.844776	71.305665
759.440306	27.845587	71.310670
758.584800	22.456434	71.315674
757.837259	28.734772	71.320679
758.097321	22.573539	71.325684
756.817180	27.500129	71.330689
756.009633	30.921253	71.335694
756.008959	15.032764	71.340698
755.145305	24.491227	71.345703
753.849282	25.140695	71.350708
753.428630	21.151968	71.355713
752.832215	23.090328	71.360718
752.507099	17.504783	71.365722
751.364467	27.652606	71.370727
750.607253	16.561583	71.375732
750.648887	22.952391	71.380737
749.494166	20.589603	71.385742
748.921691	10.960902	71.390746
748.193013	17.121122	71.395751
747.948824	22.207625	71.400756
746.779523	16.057921	71.405761
745.814821	14.588935	71.410766
745.658998	15.362799	71.415770
745.000166	30.481191	71.420775
744.255917	12.140772	71.425780
743.581253	6.836376	71.430785
742.838428	15.964956	71.435790
742.663733	14.488465	71.440794
741.528765	27.957554	71.445799
740.716419	11.641654	71.450804
740.330926	21.076030	71.455809
739.503626	20.026697	71.460814
738.744192	13.635134	71.465818
737.919792	23.013238	71.470823
737.595666	22.151867	71.475828
737.093949	34.950892	71.480833
736.550404	24.756211	71.485838
735.730310	17.759323	71.490842
734.901644	27.458215	71.495847
734.546918	18.681053	71.500852
733.738058	25.527372	71.505857
732.983109	17.326416	71.510862
732.521994	15.520229	71.515866
731.963150	24.832403	71.520871
731.231879	11.616360	71.525876
730.397745	22.240171	71.530881
729.687592	15.288858	71.535886
729.180950	18.321475	71.540890
728.084999	30.833501	71.545895
727.696975	13.313119	71.550900
727.141682	18.509074	71.555905
726.431958	12.167947	71.560910
725.566262	8.967565	71.565914
724.368162	22.071408	71.570919
724.389073	12.964800	71.575924
723.857522	17.988249	71.580929
723.538011	17.588171	71.585934
722.466815	12.402103	71.590938
721.656168	19.598774	71.595943
721.535680	11.290503	71.600948
720.394777	19.214659	71.605953
719.465548	12.402304	71.610958
719.380404	12.232981	71.615962
718.609363	18.668022	71.620967
718.280982	18.155821	71.625972
717.145632	7.837773	71.630977
716.665495	21.365024	71.635982
716.082803	18.794488	71.640986
714.608290	22.741263	71.645991
714.310296	11.980826	71.650996
713.927523	18.641041	71.656001
713.432504	31.293926	71.661006
712.778204	23.743969	71.666010
711.726728	31.988194	71.671015
711.527110	21.456504	71.676020
710.699843	20.624785	71.681025
709.495932	26.695110	71.686030
709.131879	21.051119	71.691034
708.656420	21.363391	71.696039
708.406731	7.750579	71.701044
707.563994	27.920607	71.706049
706.837260	26.538320	71.711054
706.263840	17.387575	71.716058
704.990736	24.733574	71.721063
704.772695	23.626669	71.726068
704.099505	31.192530	71.731073
702.778719	30.631770	71.736078
702.390009	26.600121	71.741082
701.848191	18.939225	71.746087
701.774819	18.220852	71.751092
700.651909	27.507730	71.756097
699.201028	31.677824	71.761102
699.099850	15.116251	71.766106
698.720798	18.671003	71.771111
698.387753	21.598719	71.776116
697.258913	17.710149	71.781121
696.664596	14.378261	71.786126
696.361493	8.953221	71.791130
695.840399	20.503281	71.796135
694.934112	18.660756	71.801140
693.815476	22.792141	71.806145
693.427441	23.945164	71.811150
692.921181	21.669955	71.816154
691.432883	16.052020	71.821159
690.993375	15.027686	71.826164
690.585961	19.652926	71.831169
690.328875	22.234249	71.836174
690.093287	11.979520	71.841178
688.971827	22.917159	71.846183
688.382615	18.073811	71.851188
687.132404	29.225911	71.856193
686.510559	22.035056	71.861198
686.196730	16.862446	71.866202
685.223431	20.445592	71.871207
684.943963	21.185532	71.876212
683.996329	24.130688	71.881217
683.216296	21.060175	71.886222
683.166072	22.287137	71.891226
682.496292	26.083719	71.896231
681.475925	20.851729	71.901236
680.491121	18.483996	71.906241
680.168246	20.870802	71.911246
679.787445	17.288888	71.916250
678.559461	22.019558	71.921255
677.850346	15.146942	71.926260
677.543482	8.085706	71.931265
676.820540	22.171989	71.936270
676.641340	15.317492	71.941274
675.254809	22.281037	71.946279
675.155743	21.047963	71.951284
674.446103	21.165729	71.956289
673.311192	14.447644	71.961294
672.871671	23.400219	71.966298
672.049574	26.196086	71.971303
671.958109	25.784931	71.976308
671.010347	17.963191	71.981313
670.050341	17.605186	71.986318
669.793765	15.772750	71.991322
668.878930	18.515578	71.996327
668.102043	7.112355	72.001332
667.434971	16.785525	72.006337
666.767232	17.607793	72.011342
666.527406	13.837862	72.016346
665.757631	18.810949	72.021351
665.039201	13.824190	72.026356
664.544322	11.733249	72.031361
663.773264	18.668175	72.036366
662.972056	25.661520	72.041370
661.992440	21.805972	72.046375
661.972860	21.009652	72.051380
661.341313	17.598551	72.056385
660.375653	18.510836	72.061390
660.056729	10.052833	72.066394
659.361955	13.664171	72.071399
658.213866	18.475162	72.076404
657.256220	17.145430	72.081409
657.116945	18.897481	72.086414
656.873228	14.883755	72.091418
655.591485	27.395424	72.096423
655.127004	16.295674	72.101428
654.334396	26.367292	72.106433
653.840974	28.295581	72.111438
652.824269	19.079829	72.116442
652.367193	23.903784	72.121447
651.946461	20.520612	72.126452
651.389692	14.861595	72.131457
650.340454	17.974321	72.136462
649.375998	13.484039	72.141466
648.850528	20.838733	72.146471
648.734139	11.356624	72.151476
648.261389	18.988337	72.156481
647.020978	25.720481	72.161486
646.675604	21.626753	72.166490
645.758111	22.471453	72.171495
644.877860	21.151477	72.176500
644.205247	25.829992	72.181505
643.613300	34.060985	72.186510
643.513726	22.537288	72.191514
642.858822	21.354885	72.196519
642.188720	14.846635	72.201524
641.062403	20.182421	72.206529
640.560589	25.035578	72.211534
639.975777	24.947404	72.216538
638.856299	23.649758	72.221543
638.782814	20.689085	72.226548
638.257797	27.420845	72.231553
637.190634	19.624442	72.236558
636.483855	24.343090	72.241562
635.700072	24.907893	72.246567
635.625098	19.274651	72.251572
634.635201	21.436538	72.256577
633.756060	21.012056	72.261582
633.570646	26.128627	72.266586
632.290853	22.458083	72.271591
631.708010	19.441338	72.276596
630.971757	20.775972	72.281601
630.461235	25.318297	72.286606
630.552493	23.037830	72.291610
629.249176	34.094339	72.296615
628.830789	14.940450	72.301620
628.281887	30.796671	72.306625
627.643704	22.886226	72.311630
626.528314	25.413438	72.316634
625.754332	24.778256	72.321639
625.605946	18.191658	72.326644
624.565511	30.463072	72.331649
623.805565	23.373073	72.336654
623.859777	18.039366	72.341658
623.168438	41.386371	72.346663
622.094948	23.634571	72.351668
621.349597	16.643172	72.356673
620.551561	17.979764	72.361678
620.442370	16.123863	72.366682
619.061332	24.272372	72.371687
618.533428	19.468163	72.376692
617.978541	33.358976	72.381697
617.416549	25.966230	72.386702
617.213712	15.600648	72.391706
616.201612	17.089597	72.396711
615.650592	22.671226	72.401716
614.871787	31.904914	72.406721
613.613409	37.972919	72.411726
613.347069	23.979586	72.416730
612.724240	22.500361	72.421735
612.288052	30.399060	72.426740
611.480674	27.481152	72.431745
610.662327	21.466428	72.436750
610.226409	21.569005	72.441754
609.673403	26.498125	72.446759
608.815951	27.976642	72.451764
608.073751	33.580839	72.456769
607.048275	30.789124	72.461774
607.210751	27.823988	72.466778
606.231972	20.853999	72.471783
605.522481	17.600400	72.476788
604.887910	31.502326	72.481793
604.168058	26.700304	72.486798
603.854597	27.428322	72.491802
602.834715	29.768454	72.496807
602.229402	19.082212	72.501812
601.924306	24.399184	72.506817
600.979520	28.848257	72.511822
600.519079	27.943962	72.516826
599.819241	31.065716	72.521831
598.852498	19.500372	72.526836
597.689767	26.325816	72.531841
597.158977	26.022478	72.536846
596.918433	23.531516	72.541850
596.421341	21.480363	72.546855
595.832427	21.736612	72.551860
594.848792	24.715916	72.556865
594.416490	24.348010	72.561870
594.047757	21.342904	72.566874
592.728955	24.350359	72.571879
592.269074	14.011528	72.576884
591.495572	20.346071	72.581889
591.111365	28.473024	72.586894
590.856838	12.673879	72.591898
589.544799	26.434552	72.596903
589.020744	28.301503	72.601908
588.409513	26.676940	72.606913
587.204848	24.457797	72.611918
586.907784	27.516982	72.616922
586.325063	23.383800	72.621927
586.037894	22.546524	72.626932
585.158069	26.106935	72.631937
584.287459	21.877686	72.636942
584.026602	10.759722	72.641946
583.164813	21.523580	72.646951
582.483991	18.155041	72.651956
582.119287	22.652071	72.656961
581.387673	21.068760	72.661966
580.471839	29.936367	72.666970
579.610167	25.767193	72.671975
579.275361	8.392928	72.676980
578.505802	27.352890	72.681985
577.662431	23.821014	72.686990
577.137624	9.643378	72.691994
576.598269	27.369827	72.696999
576.102228	26.305635	72.702004
574.973887	17.063552	72.707009
574.002908	22.049787	72.712014
573.813029	11.872954	72.717018
573.369534	23.637737	72.722023
572.561681	27.959359	72.727028
571.743233	21.227188	72.732033
571.030737	12.947000	72.737038
570.822188	29.832327	72.742042
569.554017	26.716603	72.747047
569.137079	21.680278	72.752052
568.401327	20.313663	72.757057
567.973041	23.849466	72.762062
567.673906	21.484529	72.767066
566.502115	37.517238	72.772071
566.251902	22.649336	72.777076
565.555325	21.103026	72.782081
564.428079	17.729906	72.787086
563.976010	12.957789	72.792090
563.491615	25.126461	72.797095
562.549826	19.284376	72.802100
561.945333	23.654029	72.807105
561.298136	28.653352	72.812110
560.876320	22.420956	72.817114
559.566012	19.215761	72.822119
558.884828	28.902241	72.827124
558.582208	26.919464	72.832129
557.949415	35.995875	72.837134
557.605297	24.189458	72.842138
556.679342	28.922538	72.847143
556.057390	19.122013	72.852148
555.626461	23.025651	72.857153
554.714571	31.113660	72.862158
554.129452	23.432897	72.867162
553.305577	26.330002	72.872167
553.011925	26.797840	72.877172
551.918226	26.975237	72.882177
550.921938	27.435149	72.887182
550.569907	25.182713	72.892186
549.991101	30.144338	72.897191
549.606123	29.761017	72.902196
548.955343	25.492035	72.907201
547.940547	26.921521	72.912206
547.650108	28.699231	72.917210
546.627949	33.906510	72.922215
545.852083	28.203572	72.927220
545.429594	10.743939	72.932225
545.277218	20.199536	72.937230
544.132776	18.499076	72.942234
543.086691	25.499918	72.947239
542.929956	10.760641	72.952244
542.445573	15.633109	72.957249
541.163528	30.253154	72.962254
540.990399	12.018977	72.967258
540.174708	22.351323	72.972263
539.764368	24.706346	72.977268
538.615421	12.655999	72.982273
537.795738	25.362180	72.987278
537.742417	26.435103	72.992282
537.132422	30.685797	72.997287
536.525744	18.828178	73.002292
535.536472	21.152421	73.007297
534.889539	25.945135	73.012302
534.345036	22.157523	73.017306
533.099110	28.985208	73.022311
532.458127	23.547783	73.027316
532.273756	16.205299	73.032321
531.561283	27.923052	73.037326
530.963784	19.444794	73.042330
530.076541	29.865812	73.047335
529.610866	27.405988	73.052340
529.146166	29.630907	73.057345
528.339855	22.165150	73.062350
527.830819	22.582148	73.067354
527.224842	28.205661	73.072359
525.995651	25.793346	73.077364
525.296966	14.207421	73.082369
524.241317	13.746443	73.087374
524.144506	20.356392	73.092378
523.902380	27.855196	73.097383
523.433811	28.581124	73.102388
522.413804	19.720761	73.107393
521.417378	25.652463	73.112398
521.602005	18.535039	73.117402
520.774949	22.858155	73.122407
519.845580	19.598609	73.127412
519.268143	12.832803	73.132417
518.216936	26.656028	73.137422
517.676540	15.516376	73.142426
516.789594	28.085052	73.147431
516.471758	20.970399	73.152436
515.596096	31.235043	73.157441
514.392184	32.566940	73.162446
514.495124	19.858311	73.167450
513.849606	25.123867	73.172455
513.244411	22.268400	73.177460
512.156685	13.890320	73.182465
511.904662	27.794387	73.187470
511.497162	12.428044	73.192474
510.517550	22.570477	73.197479
509.668139	26.378367	73.202484
508.997299	28.164641	73.207489
508.553177	28.883523	73.212494
508.000892	18.573626	73.217498
506.783909	25.032452	73.222503
506.416739	20.027635	73.227508
506.354738	19.488798	73.232513
504.859492	30.014561	73.237518
504.466953	25.270815	73.242522
503.746530	25.853948	73.247527
503.196113	22.598693	73.252532
502.343931	18.358658	73.257537
501.567448	23.835880	73.262542
501.356691	14.660546	73.267546
500.887407	23.980557	73.272551
500.268475	23.552516	73.277556
499.389806	29.911723	73.282561
498.469448	31.701481	73.287566
498.130664	13.282402	73.292570
497.059491	25.583975	73.297575
496.299961	21.434832	73.302580
495.889535	24.124172	73.307585
495.241407	29.785944	73.312590
494.850602	16.299732	73.317594
493.952610	27.357950	73.322599
493.438398	17.341600	73.327604
492.432246	14.934772	73.332609
491.639396	18.202248	73.337614
491.566942	7.648776	73.342618
490.386260	27.071612	73.347623
489.997793	18.687796	73.352628
489.003740	26.315847	73.357633
488.415312	19.163887	73.362638
488.084639	11.898333	73.367642
487.609300	31.692911	73.372647
486.326119	16.806678	73.377652
485.742822	17.908839	73.382657
485.138062	28.136640	73.387662
484.936897	13.089077	73.392666
483.769100	22.930354	73.397671
483.127007	19.536753	73.402676
482.640585	22.898911	73.407681
482.176969	24.961247	73.412686
481.855355	16.308176	73.417690
480.679555	17.380156	73.422695
480.293192	21.861724	73.427700
479.446464	10.811889	73.432705
478.512513	18.627474	73.437710
478.050371	2.468806	73.442714
477.464667	18.357690	73.447719
477.052529	15.108798	73.452724
475.823302	17.148031	73.457729
475.138609	25.404858	73.462734
474.959890	19.474361	73.467738
474.079269	16.729014	73.472743
473.234021	12.117321	73.477748
472.723500	17.567946	73.482753
472.125700	1.328397	73.487758
471.855829	14.062100	73.492762
470.500912	21.897448	73.497767
470.293404	7.875873	73.502772
469.852927	11.886691	73.507777
468.907285	26.435818	73.512782
468.254687	16.901970	73.517786
467.437446	26.558103	73.522791
466.883798	19.805866	73.527796
465.859922	16.236563	73.532801
465.008187	26.459559	73.537806
464.870714	22.088328	73.542810
464.437312	26.489087	73.547815
463.744014	22.012452	73.552820
462.758355	23.375831	73.557825
462.082185	18.819202	73.562830
461.886386	20.324811	73.567834
460.816181	22.978928	73.572839
460.101249	13.138065	73.577844
459.577899	13.473782	73.582849
458.957818	31.085373	73.587854
458.937037	17.380956	73.592858
457.722543	19.514039	73.597863
457.140821	17.189410	73.602868
456.138070	14.971281	73.607873
455.140739	14.404852	73.612878
454.967762	15.823251	73.617882
454.527721	24.175138	73.622887
453.627767	22.607648	73.627892
452.669479	18.319885	73.632897
451.879844	14.612351	73.637902
451.838979	5.482501	73.642906
451.151533	13.170512	73.647911
450.516329	16.816563	73.652916
449.864121	15.449290	73.657921
449.074202	24.508168	73.662926
448.391750	11.107863	73.667930
447.377269	23.069273	73.672935
446.965141	6.404351	73.677940
446.777864	9.805580	73.682945
445.471178	17.590678	73.687950
444.928236	13.225708	73.692954
444.356004	18.769743	73.697959
443.740347	12.546187	73.702964
443.218043	15.089363	73.707969
442.131529	20.519805	73.712974
442.021599	8.926843	73.717978
441.323136	23.534358	73.722983
440.104451	17.488876	73.727988
439.555073	11.828743	73.732993
438.654349	21.430374	73.737998
438.677399	11.497172	73.743002
438.064424	9.868198	73.748007
437.415924	16.518735	73.753012
436.712542	11.529658	73.758017
435.689977	22.331781	73.763022
435.101987	3.797907	73.768026
433.959765	23.563114	73.773031
433.862212	11.693804	73.778036
433.308756	12.251931	73.783041
432.291388	11.526287	73.788046
431.746402	7.877547	73.793050
431.332113	25.339655	73.798055
430.707609	21.533280	73.803060
430.044869	11.649423	73.808065
428.967615	6.905990	73.813070
428.728612	11.162242	73.818074
428.122733	12.394163	73.823079
427.431730	23.193921	73.828084
426.625701	21.163645	73.833089
425.936152	21.155285	73.838094
424.970179	12.811466	73.843098
423.726927	15.903155	73.848103
423.530334	15.004162	73.853108
423.093202	12.949803	73.858113
422.570255	14.127514	73.863118
422.454239	13.012266	73.868122
421.290236	20.396193	73.873127
420.583889	15.106410	73.878132
420.322879	13.337786	73.883137
419.176856	19.356431	73.888142
418.348116	5.036483	73.893146
417.403698	12.125235	73.898151
417.488192	14.951758	73.903156
417.018289	5.958078	73.908161
415.822426	16.139720	73.913166
415.327791	1.544203	73.918170
415.274265	17.772474	73.923175
414.514291	15.006350	73.928180
413.718116	17.859661	73.933185
412.651610	24.113208	73.938190
411.866490	10.232563	73.943194
410.803517	22.233247	73.948199
410.644853	6.977098	73.953204
410.328136	13.327204	73.958209
409.255675	20.027955	73.963214
408.651379	9.149250	73.968218
407.588297	13.968874	73.973223
407.318640	19.185597	73.978228
407.538188	15.542769	73.983233
406.576316	22.115520	73.988238
405.714798	16.962424	73.993242
404.449166	21.002236	73.998247
403.721543	16.084837	74.003252
402.832088	15.133829	74.008257
402.615552	17.420144	74.013262
402.597065	13.796323	74.018266
401.580226	16.318963	74.023271
400.830085	14.773353	74.028276
400.339202	6.886831	74.033281
399.356497	34.025324	74.038286
398.813956	-0.197775	74.043290
397.875746	18.617187	74.048295
397.253914	12.233789	74.053300
397.188208	7.540490	74.058305
396.005209	8.348741	74.063310
395.543705	22.435980	74.068314
395.153403	18.489800	74.073319
394.297761	2.084798	74.078324
393.337360	12.725641	74.083329
392.397701	10.412336	74.088334
392.164098	4.123191	74.093338
391.914694	8.237605	74.098343
390.920980	15.228572	74.103348
390.056721	15.613895	74.108353
389.446332	4.255226	74.113358
389.474527	1.284679	74.118362
387.870891	15.571251	74.123367
387.345775	12.860748	74.128372
387.106760	12.324891	74.133377
386.229151	19.437702	74.138382
385.830431	11.058704	74.143386
384.912777	14.864887	74.148391
384.501762	5.429771	74.153396
383.413085	11.172797	74.158401
382.492767	15.348394	74.163406
382.118352	12.000475	74.168410
381.549690	17.465108	74.173415
381.306923	15.245751	74.178420
380.567516	8.687140	74.183425
379.212984	7.499608	74.188430
379.205920	30.876326	74.193434
378.514025	18.798968	74.198439
377.521154	6.205062	74.203444
376.786051	14.075715	74.208449
376.207749	20.645697	74.213454
375.975136	12.900940	74.218458
375.223068	16.956694	74.223463
374.679054	15.884421	74.228468
374.378958	13.175909	74.233473
373.133850	11.184084	74.238478
372.303107	15.107303	74.243482
371.696102	17.203543	74.248487
370.692961	16.557654	74.253492
370.135131	5.684176	74.258497
369.230645	16.773411	74.263502
369.043456	7.901840	74.268506
368.788794	8.973734	74.273511
368.041874	10.212376	74.278516
366.901202	12.497732	74.283521
366.280286	20.944676	74.288526
366.143130	18.713221	74.293530
365.010610	20.975204	74.298535
363.998831	17.498632	74.303540
364.077357	10.858567	74.308545
363.248237	14.868257	74.313550
362.639946	6.672466	74.318554
361.407385	27.672590	74.323559
361.136999	19.369332	74.328564
360.865916	10.892733	74.333569
359.940125	22.366972	74.338574
358.956782	10.315575	74.343578
358.572249	2.713301	74.348583
357.871397	14.216341	74.353588
356.876843	9.330460	74.358593
355.989039	17.427293	74.363598
355.930550	1.831940	74.368602
355.728924	8.710880	74.373607
354.650336	26.594224	74.378612
354.306620	11.302922	74.383617
353.473457	9.228114	74.388622
352.635909	12.575288	74.393626
351.520089	16.777320	74.398631
351.103283	12.584652	74.403636
350.671465	16.376499	74.408641
349.866906	28.821701	74.413646
349.215102	10.368986	74.418650
348.080681	9.580033	74.423655
347.706869	12.850152	74.428660
347.781353	23.392322	74.433665
346.917151	11.815505	74.438670
346.123025	9.717133	74.443674
345.695506	14.400803	74.448679
344.472346	17.702206	74.453684
343.793063	6.477527	74.458689
343.354642	11.697494	74.463694
342.924859	9.982584	74.468698
342.009622	16.727684	74.473703
341.256014	11.106434	74.478708
340.803202	11.077716	74.483713
339.880015	15.127634	74.488718
339.133054	9.294026	74.493722
338.472597	15.106015	74.498727
337.907402	15.599805	74.503732
337.552024	24.198393	74.508737
336.709834	17.507948	74.513742
336.659776	1.455539	74.518746
335.372495	1.160861	74.523751
334.954219	11.574981	74.528756
334.096342	27.447338	74.533761
333.306915	17.116949	74.538766
333.148967	11.995253	74.543770
332.373705	15.885989	74.548775
331.376980	5.970249	74.553780
331.020292	14.119632	74.558785
329.920258	10.671334	74.563790
329.161467	6.856433	74.568794
328.442615	6.501128	74.573799
328.206386	14.205559	74.578804
327.737513	15.209099	74.583809
326.795489	12.263872	74.588814
326.381121	8.185933	74.593818
325.466833	13.666236	74.598823
324.977815	13.223843	74.603828
323.971562	0.608451	74.608833
322.904797	14.495694	74.613838
322.765830	5.236422	74.618842
322.280311	16.727227	74.623847
321.471742	30.587528	74.628852
320.895074	1.833774	74.633857
319.829508	18.861955	74.638862
319.547036	11.782711	74.643866
319.353477	11.441456	74.648871
318.552176	9.396274	74.653876
317.911426	15.023786	74.658881
316.917384	27.040322	74.663886
315.795862	4.666699	74.668890
315.247584	27.647129	74.673895
314.674821	11.468297	74.678900
314.644275	3.997264	74.683905
313.797866	11.302227	74.688910
313.100114	11.082328	74.693914
312.437245	21.975385	74.698919
311.960044	12.311148	74.703924
311.011148	12.569647	74.708929
310.029831	11.532395	74.713934
309.821266	0.740464	74.718938
309.091842	17.792340	74.723943
307.821927	13.730918	74.728948
307.256727	4.591618	74.733953
306.727952	15.292998	74.738958
306.634428	15.922922	74.743962
305.618385	9.744302	74.748967
304.897383	14.071074	74.753972
304.634118	12.375360	74.758977
304.212580	13.119061	74.763982
303.426018	13.479416	74.768986
302.282235	25.012068	74.773991
301.561763	11.343510	74.778996
300.627840	3.787814	74.784001
300.007207	19.652317	74.789006
299.766425	22.032385	74.794010
299.312592	21.306860	74.799015
298.972886	7.544504	74.804020
297.880521	13.789596	74.809025
296.945064	22.124266	74.814030
296.731372	20.363884	74.819034
295.462696	19.523817	74.824039
294.987319	29.327343	74.829044
294.664273	18.624608	74.834049
293.982585	29.884930	74.839054
293.006538	13.675769	74.844058
292.507249	15.450522	74.849063
292.020207	12.197839	74.854068
291.242412	19.061390	74.859073
290.119405	20.180235	74.864078
289.859660	18.116551	74.869082
289.311375	17.899643	74.874087
288.463735	17.474995	74.879092
287.718307	10.991490	74.884097
286.942466	18.622666	74.889102
286.653449	15.418841	74.894106
285.993049	17.850023	74.899111
284.970318	14.670107	74.904116
284.270423	14.239258	74.909121
283.731621	9.526761	74.914126
283.796231	12.837389	74.919130
282.385027	20.319114	74.924135
281.744639	17.056183	74.929140
281.384062	11.623032	74.934145
280.632536	8.291089	74.939150
279.662233	14.273895	74.944154
279.048202	14.133696	74.949159
278.422845	12.713309	74.954164
278.445255	16.014895	74.959169
277.548141	10.730339	74.964174
276.728818	13.013398	74.969178
276.288492	11.617132	74.974183
275.074521	19.182535	74.979188
274.406271	7.774785	74.984193
273.587195	18.319025	74.989198
273.404399	6.691980	74.994202
272.840540	8.043389	74.999207
271.866600	9.784998	75.004212
271.480106	9.233239	75.009217
270.797969	10.284974	75.014222
270.119372	-1.397070	75.019226
269.149001	9.723184	75.024231
268.544590	11.065290	75.029236
268.288950	4.076394	75.034241
267.201373	20.663422	75.039246
266.643003	17.426843	75.044250
265.846144	15.284781	75.049255
265.543863	13.806593	75.054260
264.649187	13.567637	75.059265
263.579540	16.557616	75.064270
263.550451	14.278984	75.069274
262.845134	16.088160	75.074279
262.207502	19.859212	75.079284
261.551669	8.178266	75.084289
260.549787	22.875164	75.089294
260.436780	8.813346	75.094298
259.479040	14.426745	75.099303
258.483091	22.616536	75.104308
257.812889	14.293457	75.109313
257.332108	18.963553	75.114318
257.125236	2.048378	75.119322
255.922327	17.709245	75.124327
255.169940	19.590578	75.129332
254.889096	6.569444	75.134337
254.463678	12.203642	75.139342
253.975396	4.897036	75.144346
252.878142	9.277487	75.149351
252.326062	10.125578	75.154356
251.481811	9.845475	75.159361
250.693333	8.667128	75.164366
250.375259	1.664536	75.169370
250.042636	13.019013	75.174375
248.746106	18.183400	75.179380
248.404578	11.072585	75.184385
247.492503	16.473716	75.189390
246.817567	4.344839	75.194394
245.768842	23.798737	75.199399
245.141852	14.029092	75.204404
245.461265	9.883086	75.209409
244.716085	19.376398	75.214414
243.913261	-4.260575	75.219418
242.992261	14.710929	75.224423
242.097032	15.542764	75.229428
241.506371	14.679797	75.234433
240.674169	17.146260	75.239438
240.344804	18.682636	75.244442
239.742299	9.962442	75.249447
238.628895	11.947057	75.254452
237.988793	2.427081	75.259457
237.210495	15.449971	75.264462
237.339860	10.347139	75.269466
236.559995	24.519824	75.274471
235.794097	8.934757	75.279476
235.273306	6.737663	75.284481
234.606517	18.008225	75.289486
233.420858	9.070350	75.294490
232.611078	13.289873	75.299495
232.172462	10.756420	75.304500
232.018125	13.873302	75.309505
231.260491	18.994367	75.314510
230.630347	9.192119	75.319514
229.570177	19.137748	75.324519
229.182647	10.511015	75.329524
228.590539	5.781802	75.334529
227.355211	8.265224	75.339534
227.070474	11.068596	75.344538
226.770372	16.257067	75.349543
225.959319	7.716773	75.354548
225.060878	9.902079	75.359553
224.363888	10.470518	75.364558
223.756019	7.530411	75.369562
222.410225	18.896603	75.374567
222.132672	13.289388	75.379572
222.114074	4.961796	75.384577
221.540469	20.181754	75.389582
220.710794	16.553221	75.394586
219.571307	0.532589	75.399591
219.156275	6.579849	75.404596
218.709418	19.057926	75.409601
217.472391	15.652020	75.414606
216.801751	11.999714	75.419610
216.274596	3.581317	75.424615
216.162148	21.919341	75.429620
215.721064	7.230204	75.434625
214.671980	14.080252	75.439630
214.150948	17.290282	75.444634
212.839065	9.380161	75.449639
212.155826	5.189001	75.454644
211.686408	7.640213	75.459649
211.345985	7.606217	75.464654
210.841260	13.169489	75.469658
209.799517	12.641778	75.474663
209.169228	9.361491	75.479668
208.606115	17.371911	75.484673
208.031786	10.427521	75.489678
207.465957	9.041816	75.494682
206.324838	16.562517	75.499687
206.013831	11.305974	75.504692
205.479554	11.287114	75.509697
204.341378	24.206548	75.514702
203.708826	17.020716	75.519706
203.406339	23.445837	75.524711
202.778926	8.480495	75.529716
201.923254	5.094224	75.534721
201.057234	8.792892	75.539726
200.690351	13.252459	75.544730
199.989175	10.525918	75.549735
199.030507	15.751576	75.554740
198.716020	12.108725	75.559745
198.149255	18.347330	75.564750
198.012318	14.822822	75.569754
196.956508	13.642959	75.574759
196.061310	9.987038	75.579764
195.736364	8.684352	75.584769
194.144815	4.515009	75.589774
193.905692	8.359728	75.594778
193.397470	26.694622	75.599783
192.997367	22.534014	75.604788
192.344410	3.338861	75.609793
190.731279	39.305852	75.614798
190.634207	13.485935	75.619802
190.409706	13.617954	75.624807
189.662226	13.547937	75.629812
189.358179	13.782519	75.634817
188.146029	14.882506	75.639822
187.512063	12.416475	75.644826
186.187353	23.115463	75.649831
185.772606	9.227915	75.654836
185.670082	0.276655	75.659841
184.681689	21.207929	75.664846
184.248499	11.924624	75.669850
183.538973	14.611230	75.674855
182.796299	18.376970	75.679860
182.457662	16.978701	75.684865
181.282545	13.673326	75.689870
180.793303	4.551919	75.694874
180.379342	12.846050	75.699879
179.759698	24.369292	75.704884
178.630482	8.074243	75.709889
177.651154	25.178598	75.714894
177.620737	15.112026	75.719898
177.245709	6.207363	75.724903
176.070526	12.902496	75.729908
175.556248	12.254437	75.734913
174.798409	24.321656	75.739918
174.873712	6.431157	75.744922
173.379372	2.801389	75.749927
172.438399	22.055204	75.754932
172.464931	9.253150	75.759937
171.976509	3.854600	75.764942
170.685344	18.025235	75.769946
170.205633	-4.248759	75.774951
169.691359	8.648468	75.779956
169.350571	10.560390	75.784961
168.228633	14.091726	75.789966
168.113109	13.801117	75.794970
167.003071	15.290089	75.799975
165.628634	10.728200	75.804980
165.460730	0.117465	75.809985
164.975242	1.369673	75.814990
164.837867	4.706189	75.819994
163.777124	8.948397	75.824999
162.853919	18.583642	75.830004
162.405620	2.818677	75.835009
161.807597	13.652528	75.840014
161.001493	5.597150	75.845018
160.167851	3.645485	75.850023
159.377857	8.052673	75.855028
159.191686	3.017499	75.860033
158.176095	16.314767	75.865038
157.532835	15.863886	75.870042
157.023410	16.572741	75.875047
156.700611	8.479726	75.880052
156.017879	2.735290	75.885057
154.803800	12.139382	75.890062
154.413431	10.609026	75.895066
153.878556	10.585542	75.900071
153.305726	10.333156	75.905076
152.529091	6.845997	75.910081
151.535425	4.199222	75.915086
151.376980	-1.059555	75.920090
150.288557	9.661685	75.925095
149.422572	3.993775	75.930100
148.962278	13.843780	75.935105
148.470818	7.039154	75.940110
148.350813	4.965824	75.945114
146.966568	14.333978	75.950119
146.457842	14.046143	75.955124
146.042775	14.350469	75.960129
145.047206	12.205443	75.965134
144.444875	7.574073	75.970138
143.759660	10.602147	75.975143
143.473865	12.825408	75.980148
142.676841	14.523088	75.985153
141.628625	17.252671	75.990158
141.506721	14.381748	75.995162
140.951097	1.653606	76.000167
139.490038	15.744112	76.005172
139.074577	9.308971	76.010177
138.480330	12.125434	76.015182
138.138692	1.936620	76.020186
137.129505	10.688340	76.025191
136.367849	7.988809	76.030196
136.104983	4.974794	76.035201
135.248764	11.675852	76.040206
134.613415	1.866590	76.045210
133.839751	6.329525	76.050215
133.112548	14.102781	76.055220
133.111827	13.106355	76.060225
131.609462	27.269690	76.065230
131.113541	16.268151	76.070234
130.824757	9.551054	76.075239
130.490074	14.648855	76.080244
129.603543	24.342918	76.085249
129.127869	14.610685	76.090254
128.137321	7.508774	76.095258
127.538278	4.155724	76.100263
126.261510	5.769065	76.105268
126.209667	15.905586	76.110273
125.141938	-0.730366	76.115278
124.353241	25.366431	76.120282
123.771401	9.485579	76.125287
123.312912	10.594727	76.130292
123.307159	4.939463	76.135297
121.900870	11.261483	76.140302
121.233999	3.868281	76.145306
120.701376	9.235750	76.150311
120.176355	15.369945	76.155316
119.531891	12.114020	76.160321
118.483495	0.658150	76.165326
118.305211	9.554912	76.170330
117.796454	10.711498	76.175335
116.604287	25.520773	76.180340
116.372802	10.635827	76.185345
115.660030	18.796275	76.190350
114.344026	12.485814	76.195354
113.624970	5.621301	76.200359
112.875097	7.384007	76.205364
112.727418	16.588113	76.210369
112.332541	4.884539	76.215374
112.107367	11.152259	76.220378
110.503367	21.247721	76.225383
110.118223	12.002504	76.230388
110.015280	7.464968	76.235393
108.876453	20.159041	76.240398
107.954787	12.081110	76.245402
107.577086	7.533774	76.250407
106.960796	7.122759	76.255412
106.501296	9.853089	76.260417
105.403595	14.315668	76.265422
104.897990	14.456252	76.270426
104.213544	15.404327	76.275431
103.110734	7.987609	76.280436
102.712825	8.292360	76.285441
101.812786	11.720534	76.290446
101.507031	12.395345	76.295450
101.513274	5.758935	76.300455
100.521036	7.675404	76.305460
99.667862	16.254036	76.310465
99.204199	19.190026	76.315470
98.005825	-5.459207	76.320474
97.405470	20.400980	76.325479
96.775966	21.663553	76.330484
96.589984	2.972691	76.335489
95.178830	6.047156	76.340494
94.553604	18.034892	76.345498
94.234406	15.774145	76.350503
93.907167	10.960157	76.355508
93.656075	-1.166859	76.360513
92.661425	6.950232	76.365518
91.785440	12.102818	76.370522
90.616437	4.450674	76.375527
89.615820	20.415210	76.380532
89.766175	9.080407	76.385537
88.852783	10.773008	76.390542
89.046334	2.750626	76.395546
88.429593	16.662362	76.400551
87.175150	13.267189	76.405556
86.516528	8.381476	76.410561
85.317670	15.340605	76.415566
85.012228	14.370696	76.420570
84.857622	15.699459	76.425575
83.520684	13.337675	76.430580
82.953104	15.421385	76.435585
82.445883	13.230046	76.440590
81.995462	9.700352	76.445594
81.530240	11.411367	76.450599
80.489279	11.255728	76.455604
80.060626	-0.688436	76.460609
79.046185	13.013921	76.465614
78.066432	-0.043930	76.470618
77.263992	10.461426	76.475623
76.911787	9.164681	76.480628
76.860336	1.544051	76.485633
76.074489	21.298238	76.490638
75.240533	7.136978	76.495642
74.498766	9.227968	76.500647
73.798744	16.828179	76.505652
73.604381	12.116000	76.510657
72.259513	21.944666	76.515662
71.630888	15.920404	76.520666
71.054484	16.718801	76.525671
70.355746	12.579039	76.530676
69.322950	5.099139	76.535681
68.923978	14.535694	76.540686
68.728191	7.081574	76.545690
68.302464	10.405734	76.550695
67.740899	8.385482	76.555700
66.932329	1.267197	76.560705
66.123466	5.647459	76.565710
65.127872	10.599943	76.570714
64.231170	15.501967	76.575719
63.832684	11.948225	76.580724
63.710132	1.576266	76.585729
62.234649	17.949254	76.590734
61.573708	4.492077	76.595738
61.099262	6.783276	76.600743
60.649082	10.366788	76.605748
60.399093	4.034582	76.610753
59.163535	12.945426	76.615758
58.657487	11.572299	76.620762
58.028720	-1.502094	76.625767
57.334086	12.798934	76.630772
56.810159	0.471024	76.635777
55.734214	14.337729	76.640782
55.263790	11.795195	76.645786
54.975378	10.909302	76.650791
53.662733	20.078437	76.655796
53.179180	11.661016	76.660801
52.528593	19.412613	76.665806
52.315244	11.600192	76.670810
51.513134	13.251405	76.675815
50.416171	5.018546	76.680820
50.013846	28.213797	76.685825
49.701686	8.089194	76.690830
48.743045	6.340421	76.695834
47.776916	12.267446	76.700839
47.311212	1.388853	76.705844
47.154754	6.817760	76.710849
46.295431	17.871488	76.715854
45.269076	9.513833	76.720858
45.118996	2.828248	76.725863
44.069522	22.148271	76.730868
43.580857	10.483325	76.735873
42.854684	21.132642	76.740878
42.457541	14.415496	76.745882
41.440602	12.704407	76.750887
40.463413	15.829533	76.755892
40.016585	13.215433	76.760897
39.746671	22.402766	76.765902
38.491247	18.749168	76.770906
37.939610	12.928671	76.775911
37.399705	17.565653	76.780916
37.342669	9.840262	76.785921
36.182808	16.082027	76.790926
35.167434	20.663962	76.795930
34.594727	14.876786	76.800935
34.279075	17.284582	76.805940
34.411129	4.129849	76.810945
33.018424	13.406370	76.815950
32.346769	12.726675	76.820954
31.407284	17.741184	76.825959
30.474915	9.529387	76.830964
29.939894	8.039469	76.835969
29.599934	10.474795	76.840974
29.563831	5.404664	76.845978
28.511235	10.005150	76.850983
27.655707	14.266719	76.855988
27.200653	2.090250	76.860993
25.905239	11.346525	76.865998
25.621039	15.223674	76.871002
24.682013	14.706468	76.876007
24.242757	15.427810	76.881012
23.979264	6.344557	76.886017
22.651953	17.342052	76.891022
21.744633	10.543866	76.896026
21.428936	19.203942	76.901031
20.846013	15.487247	76.906036
20.770712	4.768730	76.911041
19.697625	11.069194	76.916046
19.154387	7.371402	76.921050
18.908694	9.376978	76.926055
17.544921	14.337744	76.931060
16.893341	7.907180	76.936065
16.410585	11.989453	76.941070
15.997830	5.735252	76.946074
14.776326	16.075666	76.951079
13.948811	14.845281	76.956084
14.017989	9.797779	76.961089
13.410689	22.205269	76.966094
12.486613	13.895967	76.971098
11.728171	19.703153	76.976103
11.283940	28.028941	76.981108
10.408384	21.082193	76.986113
9.320257	20.848957	76.991118
8.850185	10.664887	76.996122
8.749154	7.036907	77.001127
8.026998	22.934973	77.006132
7.082981	10.538466	77.011137
6.293249	18.397414	77.016142
5.810660	16.151704	77.021147
5.610520	11.758982	77.026151
4.332580	10.814898	77.031156
3.957697	14.727012	77.036161