Tue Jun 21 13:30:14 2022

Number of Points = 9930

Depth (nm)	Load (N)	Time (s)
0.855842	122.408185	0.000000
0.521101	110.021109	0.005005
0.232723	99.292264	0.010010
0.397467	90.049507	0.015014
-0.037391	83.313520	0.020019
-0.135239	72.793497	0.025024
-0.415613	58.247702	0.030029
-0.880806	47.305253	0.035034
-0.802200	35.312540	0.040038
-1.128325	26.174980	0.045043
-1.282141	14.812967	0.050048
-1.843309	9.000334	0.055053
-2.344724	-2.338443	0.060058
-2.396862	-4.458994	0.065062
-2.847781	-1.549398	0.070067
-3.279191	-14.135657	0.075072
-3.641195	-10.445928	0.080077
-3.587928	-6.417667	0.085082
-3.691279	-8.914339	0.090086
-4.520402	4.608698	0.095091
-5.037971	-3.014380	0.100096
-5.059227	2.401833	0.105101
-5.461530	1.324747	0.110106
-5.050976	-7.759151	0.115110
-5.303530	-0.850885	0.120115
-5.538824	-0.281846	0.125120
-5.802076	-2.088409	0.130125
-6.251248	-3.090048	0.135130
-6.458848	-10.287693	0.140134
-6.861156	0.153756	0.145139
-7.143447	-0.605763	0.150144
-7.810181	-3.340073	0.155149
-8.480677	0.267937	0.160154
-7.757256	-5.133436	0.165158
-8.369192	1.458223	0.170163
-8.645961	-4.147528	0.175168
-8.552504	-0.939329	0.180173
-8.898329	3.177122	0.185178
-8.375819	-7.464515	0.190182
-9.266637	-0.129103	0.195187
-9.935445	0.609995	0.200192
-9.928387	-3.001542	0.205197
-10.223117	-7.592788	0.210202
-10.008017	-5.909989	0.215206
-10.497561	-7.399262	0.220211
-10.512176	-7.890331	0.225216
-11.464746	-13.064493	0.230221
-11.733765	-1.646217	0.235226
-11.676970	-7.759885	0.240230
-12.140198	-2.140050	0.245235
-11.775251	-10.849157	0.250240
-11.492845	-10.491742	0.255245
-12.560881	-5.274365	0.260250
-12.860119	-10.379311	0.265254
-13.305609	-9.900969	0.270259
-13.618394	-9.176622	0.275264
-13.427330	-1.438425	0.280269
-14.234130	5.495318	0.285274
-14.553150	-14.687934	0.290278
-14.897755	0.060620	0.295283
-15.244038	-8.529531	0.300288
-14.853939	-3.911570	0.305293
-14.902049	-10.210921	0.310298
-14.557619	-15.323982	0.315302
-14.992967	-2.725147	0.320307
-15.427241	-0.058855	0.325312
-16.012950	-17.185649	0.330317
-16.469280	-0.270428	0.335322
-16.575225	-10.649340	0.340326
-17.460355	-1.642274	0.345331
-17.554678	-14.609750	0.350336
-17.476677	-14.831010	0.355341
-18.002692	-10.554682	0.360346
-17.909949	-14.581385	0.365350
-18.194283	-15.092713	0.370355
-17.894436	-17.529857	0.375360
-18.172910	-8.387637	0.380365
-18.831120	-2.881935	0.385370
-19.069086	-8.140884	0.390374
-19.163238	-7.625999	0.395379
-19.328522	-12.450220	0.400384
-19.516878	-6.282325	0.405389
-20.762111	-10.500685	0.410394
-21.118092	-13.005842	0.415398
-21.113581	-2.852577	0.420403
-21.277779	-17.307817	0.425408
-20.956908	-12.945782	0.430413
-21.319346	-1.193146	0.435418
-21.111299	-13.130689	0.440422
-21.061317	-7.008576	0.445427
-22.038046	-12.232804	0.450432
-22.550855	-14.205635	0.455437
-22.985808	-14.635781	0.460442
-22.602283	-15.101612	0.465446
-23.166869	-2.846442	0.470451
-23.549192	-12.401895	0.475456
-24.161923	-8.353335	0.480461
-24.263819	-7.284635	0.485466
-24.033814	-14.153563	0.490470
-24.575814	-14.383844	0.495475
-24.434340	-10.451098	0.500480
-24.254575	-9.257953	0.505485
-24.878603	-10.136704	0.510490
-25.335308	-22.014283	0.515494
-25.872251	-11.687694	0.520499
-25.915262	-8.773025	0.525504
-26.409448	-6.671644	0.530509
-26.555978	-6.351734	0.535514
-26.321690	-23.867483	0.540518
-27.258005	-5.287412	0.545523
-27.347674	-18.588555	0.550528
-27.648906	-16.477687	0.555533
-27.778034	-3.541210	0.560538
-27.553077	-17.465931	0.565542
-27.987459	-23.215280	0.570547
-27.990517	-8.624328	0.575552
-28.327499	-16.249081	0.580557
-28.878906	-10.193142	0.585562
-28.786991	-15.209925	0.590566
-29.540296	-10.298237	0.595571
-29.760129	-17.127797	0.600576
-30.345578	-11.248163	0.605581
-30.492287	-9.372055	0.610586
-30.480858	-16.411788	0.615590
-30.809203	-5.483339	0.620595
-30.523124	-14.892151	0.625600
-30.908393	-8.456428	0.630605
-31.361950	-0.795796	0.635610
-31.520102	-11.294524	0.640614
-31.979764	-3.328397	0.645619
-31.936874	-5.635771	0.650624
-32.123521	-13.538794	0.655629
-33.232636	-5.951548	0.660634
-33.579296	-4.646957	0.665638
-33.912832	-0.221939	0.670643
-33.428356	-7.668176	0.675648
-33.348371	-15.380131	0.680653
-33.990730	-7.602989	0.685658
-33.748945	-11.252603	0.690662
-34.352149	-5.607615	0.695667
-34.604507	-5.002202	0.700672
-35.231800	-0.875846	0.705677
-35.851249	-0.962074	0.710682
-35.966272	-5.233995	0.715686
-36.062919	-3.160950	0.720691
-35.848476	-8.520072	0.725696
-35.742322	-1.568594	0.730701
-36.028700	0.103513	0.735706
-35.887221	-8.127945	0.740710
-36.789521	-15.445962	0.745715
-36.909584	-9.204130	0.750720
-37.258565	-5.011185	0.755725
-38.243921	-2.134839	0.760730
-38.384640	-10.602738	0.765734
-38.343278	-8.680616	0.770739
-38.616967	-3.224578	0.775744
-39.076394	-11.559385	0.780749
-39.239081	-9.743974	0.785754
-38.738471	-9.070653	0.790758
-38.874041	-11.919358	0.795763
-39.285407	-7.129411	0.800768
-40.110877	-12.935556	0.805773
-40.663173	-10.907036	0.810778
-40.326017	-16.578332	0.815782
-40.770383	-7.151319	0.820787
-40.740526	-4.412898	0.825792
-40.764774	-13.626662	0.830797
-41.765664	-2.199475	0.835802
-42.137975	-14.399660	0.840806
-42.258489	-10.344992	0.845811
-42.252792	-9.019817	0.850816
-42.313023	-4.609670	0.855821
-42.400222	-8.860149	0.860826
-42.522976	-10.036210	0.865830
-43.171771	-4.597186	0.870835
-43.584028	-4.510327	0.875840
-43.398806	-8.101045	0.880845
-43.644782	-7.880698	0.885850
-43.895914	-11.987207	0.890854
-44.759093	-1.199686	0.895859
-44.780618	-3.676163	0.900864
-44.831516	-3.822009	0.905869
-44.749456	-2.224924	0.910874
-44.968114	-15.916343	0.915878
-46.061347	-1.914651	0.920883
-46.487492	-2.819459	0.925888
-46.485292	-3.864267	0.930893
-46.557209	-0.595334	0.935898
-46.352056	-17.776716	0.940902
-46.569966	-4.164080	0.945907
-47.367799	-9.299527	0.950912
-47.752719	-7.488360	0.955917
-48.201505	-0.280015	0.960922
-48.005213	-5.954431	0.965926
-48.050480	-7.921014	0.970931
-48.132979	-13.536432	0.975936
-48.300031	-6.373166	0.980941
-49.118003	-5.902993	0.985946
-49.520502	-9.717840	0.990950
-49.604399	-1.712706	0.995955
-49.692862	-5.958832	1.000960
-49.639504	-17.745051	1.005965
-49.941069	-6.124058	1.010970
-50.711235	-16.417041	1.015974
-51.280382	-7.972210	1.020979
-51.391600	-5.533067	1.025984
-51.305626	-11.789105	1.030989
-51.570438	-5.373131	1.035994
-51.044767	-16.848425	1.040998
-51.283258	-11.977785	1.046003
-51.763219	-15.662783	1.051008
-52.366430	-18.855745	1.056013
-53.324458	-14.442754	1.061018
-53.386829	-7.743784	1.066022
-53.441036	-6.065329	1.071027
-53.132557	-15.605918	1.076032
-53.510496	-15.407131	1.081037
-54.361736	-6.022455	1.086042
-54.550741	-17.021634	1.091046
-54.783449	-4.293164	1.096051
-54.954598	-3.692318	1.101056
-54.615415	-7.685043	1.106061
-54.646707	-1.750949	1.111066
-55.422346	-12.343170	1.116070
-55.773387	-10.083156	1.121075
-56.134382	-6.156001	1.126080
-56.029421	-6.362387	1.131085
-56.406545	-2.916422	1.136090
-56.542911	-13.163798	1.141094
-57.042200	-5.112571	1.146099
-57.767124	-15.539535	1.151104
-57.684536	-9.640484	1.156109
-58.121459	-3.116482	1.161114
-57.528885	-22.387244	1.166118
-57.786530	-12.440597	1.171123
-58.294977	-14.467424	1.176128
-58.886207	-12.138428	1.181133
-59.430982	-13.744446	1.186138
-59.386869	-22.708058	1.191142
-59.723492	-10.016454	1.196147
-59.421656	-10.467773	1.201152
-59.358136	-16.251227	1.206157
-60.168162	-15.599045	1.211162
-60.603834	-15.112852	1.216166
-60.916679	-9.692955	1.221171
-61.128991	-9.006754	1.226176
-60.964796	-10.796482	1.231181
-61.379371	-16.715263	1.236186
-61.866940	-21.608649	1.241190
-62.373268	-17.244807	1.246195
-62.547017	-16.204464	1.251200
-62.632080	-18.563067	1.256205
-62.778650	-5.995286	1.261210
-62.505148	-9.205957	1.266214
-62.673069	0.572710	1.271219
-63.598119	-4.642110	1.276224
-63.737727	-16.996462	1.281229
-64.248234	-2.137955	1.286234
-64.119052	-5.828913	1.291238
-64.296083	-7.799328	1.296243
-64.679321	-5.283367	1.301248
-65.244759	-12.290715	1.306253
-65.962224	-10.645095	1.311258
-65.989631	-14.748198	1.316262
-66.151882	-7.485680	1.321267
-65.879020	-11.651731	1.326272
-65.812893	-7.653033	1.331277
-66.120988	-5.581872	1.336282
-66.458471	-15.523620	1.341286
-67.270553	-4.677863	1.346291
-67.552007	-17.092788	1.351296
-67.522684	-16.109163	1.356301
-67.563010	-9.261109	1.361306
-67.451699	-18.141131	1.366310
-68.238734	-11.377409	1.371315
-68.746420	-10.036282	1.376320
-68.730395	-16.695724	1.381325
-69.298953	3.087175	1.386330
-69.047453	-12.164074	1.391334
-69.216476	-10.928760	1.396339
-69.589061	-5.369912	1.401344
-69.697574	-9.566342	1.406349
-70.491897	-0.049205	1.411354
-70.465769	-5.724448	1.416358
-70.614630	-0.855427	1.421363
-71.444148	3.856365	1.426368
-71.817478	-2.226327	1.431373
-72.009556	-10.136539	1.436378
-71.731138	-6.124058	1.441382
-72.221771	0.378649	1.446387
-71.932876	-6.053469	1.451392
-72.012377	-10.124266	1.456397
-72.167885	-7.001134	1.461402
-73.017592	-9.062022	1.466406
-73.657809	-6.858308	1.471411
-73.867677	-3.462734	1.476416
-73.813188	-9.306459	1.481421
-74.341164	2.038867	1.486426
-73.863909	-5.180625	1.491430
-74.174188	-0.418269	1.496435
-74.940312	-2.929697	1.501440
-75.019491	-10.360338	1.506445
-75.456393	-2.203606	1.511450
-75.182411	-4.574311	1.516454
-75.360189	-7.632499	1.521459
-76.346122	-8.017570	1.526464
-76.711993	-3.664749	1.531469
-77.208160	-1.532447	1.536474
-76.881604	-2.431664	1.541478
-76.855951	-1.319163	1.546483
-76.902345	-6.996407	1.551488
-77.297087	-4.894320	1.556493
-77.869111	-9.524095	1.561498
-78.444739	-3.579382	1.566502
-78.532785	-5.877503	1.571507
-78.565842	-10.998699	1.576512
-78.651365	-13.286581	1.581517
-78.771656	-8.892932	1.586522
-78.850736	-9.761873	1.591526
-79.630147	-0.095653	1.596531
-79.610832	-5.990189	1.601536
-79.780504	-12.698798	1.606541
-80.273491	5.709596	1.611546
-80.439764	-14.452756	1.616550
-81.148635	-9.120602	1.621555
-81.627734	-4.081649	1.626560
-81.686051	-4.786889	1.631565
-81.832807	-5.966275	1.636570
-81.830974	-9.011781	1.641574
-81.750641	-5.784639	1.646579
-82.164952	-0.846004	1.651584
-81.967125	-10.821939	1.656589
-82.785139	-13.234786	1.661594
-83.383342	-8.196041	1.666598
-83.349943	-9.559182	1.671603
-83.567164	-9.057857	1.676608
-83.395007	-10.166922	1.681613
-84.079838	-3.551544	1.686618
-84.764391	-5.018576	1.691622
-84.621149	-11.188587	1.696627
-85.252900	-1.623978	1.701632
-85.295383	-7.473153	1.706637
-85.706183	-6.883135	1.711642
-85.215260	-17.931762	1.716646
-85.572522	1.194937	1.721651
-85.365133	-17.206724	1.726656
-86.273957	-9.766303	1.731661
-86.745048	-4.700458	1.736666
-86.884805	-7.215764	1.741670
-87.050955	-8.389965	1.746675
-87.062062	-6.201241	1.751680
-87.179581	-8.872176	1.756685
-88.368127	-5.915008	1.761690
-88.493118	-13.233869	1.766694
-88.553100	-10.134648	1.771699
-88.395825	-1.159705	1.776704
-88.198306	-7.806582	1.781709
-89.145034	-0.724156	1.786714
-89.515685	-0.904268	1.791718
-89.965952	-1.505919	1.796723
-90.228118	-1.564088	1.801728
-89.939375	-5.256606	1.806733
-90.230604	4.223789	1.811738
-90.411417	-6.028855	1.816742
-90.211311	-2.544691	1.821747
-90.995608	0.549968	1.826752
-91.432806	-12.181142	1.831757
-91.911302	-4.818102	1.836762
-91.879640	-9.300395	1.841766
-91.947788	0.744130	1.846771
-92.185674	-2.881697	1.851776
-92.367918	-15.114729	1.856781
-93.125111	0.906274	1.861786
-92.999767	-9.456665	1.866790
-93.285386	-1.122325	1.871795
-93.891457	-1.352841	1.876800
-93.492906	-14.290634	1.881805
-93.745507	-8.072635	1.886810
-94.643812	-4.683619	1.891814
-94.720403	-1.967827	1.896819
-95.009132	-7.760039	1.901824
-95.120713	-8.560648	1.906829
-95.463969	-2.959889	1.911834
-95.000597	-6.481626	1.916838
-95.699739	-5.258170	1.921843
-96.283124	-11.424270	1.926848
-96.591222	-7.347613	1.931853
-96.830079	-12.685337	1.936858
-96.510409	-9.916377	1.941862
-96.740667	-6.564194	1.946867
-97.069212	-5.042770	1.951872
-97.485922	-11.743815	1.956877
-98.011070	1.176548	1.961882
-98.074021	-2.079637	1.966886
-98.314416	-9.874297	1.971891
-98.413825	-14.103607	1.976896
-99.010801	-1.897142	1.981901
-99.847570	1.875562	1.986906
-99.396074	-4.749047	1.991910
-99.555949	-4.872107	1.996915
-99.283627	-4.852785	2.006912
-99.848818	-2.878679	2.016909
-99.301986	-7.849920	2.026906
-98.466122	-3.675763	2.036902
-98.295565	-6.797526	2.046899
-97.151783	-5.777644	2.056896
-97.056911	-2.953574	2.066893
-97.010809	-7.143423	2.076890
-95.973582	-8.398480	2.086886
-95.522062	-5.491213	2.096883
-95.423835	-7.750589	2.106880
-94.595065	-4.951045	2.116877
-94.164207	-9.109180	2.126874
-93.330748	-6.049007	2.136870
-92.779481	-9.393270	2.146867
-92.477601	-9.684633	2.156864
-92.548728	-7.348771	2.166861
-91.401348	-0.846876	2.176858
-91.038749	-3.267598	2.186854
-90.525052	-5.961709	2.196851
-89.716852	-3.620713	2.206848
-89.514073	-10.777768	2.216845
-89.377394	-7.649029	2.226842
-88.479467	-12.366622	2.236838
-88.032038	-5.789118	2.246835
-87.663894	-3.807759	2.256832
-86.822790	-9.085186	2.266829
-86.248107	-6.619765	2.276826
-86.072343	-14.735180	2.286822
-85.784049	-3.378597	2.296819
-84.769421	-10.585929	2.306816
-84.888785	-2.009042	2.316813
-84.114043	-10.338846	2.326810
-83.636347	-13.463064	2.336806
-82.796794	-3.247940	2.346803
-82.037924	-7.022941	2.356800
-81.873253	-6.639152	2.366797
-81.808641	-3.048970	2.376794
-81.505804	-5.400716	2.386790
-80.803369	-4.576456	2.396787
-79.615813	-6.694958	2.406784
-78.985129	-9.083412	2.416781
-79.004276	-10.673293	2.426778
-78.438084	-6.177063	2.436774
-78.435295	-3.903430	2.446771
-77.349154	-9.054278	2.456768
-77.312742	-12.307744	2.466765
-76.695718	-9.658861	2.476762
-76.078996	-1.753359	2.486758
-75.391938	-7.340182	2.496755
-74.747125	-4.886965	2.506752
-74.076678	-8.325652	2.516749
-74.109312	-12.829860	2.526746
-74.047136	-7.463178	2.536742
-72.874739	-3.492739	2.546739
-72.584273	-7.545822	2.556736
-71.863379	-11.925466	2.566733
-71.278598	-9.010232	2.576730
-71.209120	-12.465772	2.586726
-70.670251	-13.227709	2.596723
-69.850472	-8.456546	2.606720
-69.849799	-2.335766	2.616717
-68.997071	-6.860142	2.626714
-68.313484	-7.144770	2.636710
-68.082575	-10.827593	2.646707
-67.055369	-11.343198	2.656704
-66.692216	-6.849105	2.666701
-66.677842	-8.373012	2.676698
-66.370528	-1.475327	2.686694
-65.200978	-6.864048	2.696691
-64.797598	-7.978565	2.706688
-64.780436	-7.649382	2.716685
-64.213174	-5.020905	2.726682
-63.336924	-7.398652	2.736678
-62.769694	-6.953492	2.746675
-62.029435	-2.546348	2.756672
-61.455690	-5.249214	2.766669
-61.909187	-6.691095	2.776666
-61.458773	0.907835	2.786662
-60.269962	-6.423972	2.796659
-60.126185	-5.376391	2.806656
-59.415634	-10.316649	2.816653
-58.464224	-10.423937	2.826650
-58.549614	-9.528680	2.836646
-58.238170	-6.306180	2.846643
-57.318600	-4.542195	2.856640
-56.976635	-4.377250	2.866637
-56.786876	-5.823900	2.876634
-55.757132	-8.481554	2.886630
-55.486906	-14.132123	2.896627
-55.089580	-8.277185	2.906624
-53.909642	-7.217044	2.916621
-53.946953	0.797959	2.926618
-53.690069	-5.426168	2.936614
-52.685751	-10.475930	2.946611
-52.081307	-9.102549	2.956608
-51.997668	-3.295048	2.966605
-51.929172	-5.890731	2.976602
-50.981768	-12.980229	2.986598
-50.585078	-14.782419	2.996595
-49.432085	-13.153708	3.006592
-49.397721	-17.454433	3.016589
-49.186628	-6.108178	3.026586
-48.702472	-8.315678	3.036582
-47.419908	-7.214043	3.046579
-47.304439	-10.283214	3.056576
-47.296110	-10.004731	3.066573
-46.413855	-7.912697	3.076570
-46.107571	-5.155248	3.086566
-45.523955	-8.976501	3.096563
-44.621908	-9.668368	3.106560
-44.591588	-5.281175	3.116557
-43.962542	-9.790832	3.126554
-43.342132	-6.649330	3.136550
-43.362638	-5.866575	3.146547
-42.298819	-0.208545	3.156544
-41.651745	-6.108833	3.166541
-41.558995	-9.938898	3.176538
-40.984050	-10.515345	3.186534
-40.040690	-7.865568	3.196531
-40.345050	-9.509383	3.206528
-39.269665	-12.710443	3.216525
-38.626746	-2.060261	3.226522
-38.248789	-10.625871	3.236518
-38.072456	-10.891104	3.246515
-37.446351	-16.027408	3.256512
-36.641906	-7.291117	3.266509
-36.334084	-10.676467	3.276506
-36.147889	-13.405054	3.286502
-35.590871	-12.704894	3.296499
-34.921030	-12.752311	3.306496
-33.980035	-13.825841	3.316493
-33.485854	-11.642472	3.326490
-33.289034	-11.910900	3.336486
-33.107448	-13.089652	3.346483
-32.656000	-15.897334	3.356480
-31.635967	-4.900598	3.366477
-31.521679	-8.723758	3.376474
-31.002712	-7.613431	3.386470
-30.314178	-10.361581	3.396467
-30.036834	-12.659508	3.406464
-29.284468	-5.264100	3.416461
-28.420690	-11.185648	3.426458
-28.268076	-6.211328	3.436454
-28.306083	-14.106405	3.446451
-27.369652	-5.328937	3.456448
-27.216764	-9.086568	3.466445
-26.303556	-5.426082	3.476442
-25.835789	-8.617214	3.486438
-25.224702	-7.885699	3.496435
-25.041292	-9.576105	3.506432
-24.107655	-8.056287	3.516429
-23.862913	-7.971859	3.526426
-23.675097	-7.378706	3.536422
-22.420883	-11.985956	3.546419
-22.405563	-7.260185	3.556416
-22.352121	-5.586906	3.566413
-20.798137	-6.863103	3.576410
-20.858215	-6.915511	3.586406
-20.830566	-9.993257	3.596403
-19.723230	-10.546028	3.606400
-19.401738	-14.120358	3.616397
-19.029014	-9.574496	3.626394
-18.082405	-8.781569	3.636390
-17.488838	-11.218205	3.646387
-17.642024	-5.855374	3.656384
-17.144735	-4.468787	3.666381
-16.091891	-11.367682	3.676378
-16.064543	-5.348530	3.686374
-15.104199	-11.264135	3.696371
-14.292318	-12.994394	3.706368
-14.581207	-17.672330	3.716365
-14.087527	-7.285314	3.726362
-13.064459	-11.274569	3.736358
-12.881702	-16.434273	3.746355
-12.712966	-15.708541	3.756352
-11.398818	-16.616238	3.766349
-11.103825	-12.332148	3.776346
-11.423957	-10.316042	3.786342
-10.297747	-5.137997	3.796339
-9.370580	-10.328697	3.806336
-9.295303	-5.896389	3.816333
-9.253421	-10.378363	3.826330
-8.518629	-3.731063	3.836326
-7.856444	-2.575095	3.846323
-7.012002	-0.793520	3.856320
-6.447811	-1.217227	3.866317
-6.659484	-3.883686	3.876314
-6.094591	-3.448801	3.886310
-5.055115	0.092188	3.896307
-4.864885	-8.059219	3.906304
-4.342078	-4.963787	3.916301
-3.432042	0.489928	3.926298
-3.187455	-1.705363	3.936294
-3.322798	0.601617	3.946291
-2.644067	9.354595	3.956288
-2.050567	16.061856	3.966285
-1.858862	31.278117	3.976282
-1.321608	51.855788	3.986278
-0.942570	62.574814	3.996275
-0.602718	88.192068	4.006272
-0.262152	107.929048	4.016269
0.000000	129.726874	4.021274
0.196864	134.451864	4.026278
0.369582	163.299946	4.031283
0.649450	171.687757	4.036288
0.936322	180.970711	4.041293
0.995712	195.537706	4.046298
1.142552	197.124875	4.051302
1.239362	205.486974	4.056307
1.448538	211.054941	4.061312
1.271170	210.127469	4.066317
1.041284	215.272236	4.071322
1.346110	220.679720	4.076326
1.468157	212.216728	4.081331
1.175276	227.802322	4.086336
1.725684	230.223114	4.091341
1.834587	235.283174	4.096346
1.594403	226.629143	4.101350
1.553526	225.341822	4.106355
1.625594	226.452180	4.111360
1.510212	217.891549	4.116365
1.534302	225.545226	4.121370
1.671807	227.534142	4.126374
1.921182	235.470007	4.131379
1.786765	226.668813	4.136384
1.616289	212.742071	4.141389
1.294878	220.104263	4.146394
1.525952	230.520513	4.151398
1.740302	240.393312	4.156403
1.692825	236.961248	4.161408
1.963494	239.158210	4.166413
1.471055	244.561163	4.171418
1.735498	242.767831	4.176422
1.799238	241.157709	4.181427
1.744808	245.705104	4.186432
1.813356	239.685889	4.191437
1.582840	243.546308	4.196442
1.715259	232.789328	4.201446
1.745764	247.661501	4.206451
1.761846	244.119059	4.211456
1.783512	237.868634	4.216461
1.600930	241.645732	4.221466
1.710424	233.667294	4.226470
1.307942	239.229006	4.231475
1.473913	244.106358	4.236480
1.866517	240.513607	4.241485
1.848640	245.921650	4.246490
1.850682	248.312872	4.251494
2.218926	268.207986	4.256499
2.016833	261.919813	4.261504
2.081532	242.558526	4.266509
1.771773	252.716244	4.271514
1.731099	245.687977	4.276518
1.946825	274.247940	4.281523
2.197426	273.614869	4.286528
2.086328	267.511133	4.291533
2.113783	273.261754	4.296538
2.302222	267.747000	4.301542
2.307803	252.951401	4.306547
1.983515	253.484272	4.311552
2.160665	249.096015	4.316557
1.925881	255.906928	4.321562
2.315521	248.497981	4.326566
2.155885	244.989766	4.331571
1.905770	244.352386	4.336576
1.813306	256.032293	4.341581
1.754961	272.902434	4.346586
2.437669	275.883272	4.351590
2.583514	279.620007	4.356595
2.272319	278.848485	4.361600
2.753303	275.252340	4.366605
1.811687	266.150250	4.371610
2.395439	271.741068	4.376614
2.345198	259.394775	4.381619
1.879912	269.033609	4.386624
2.210647	269.063344	4.391629
2.097938	281.059203	4.396634
2.347888	275.661741	4.401638
2.409411	288.915786	4.406643
2.432803	284.204679	4.411648
2.435807	288.333497	4.416653
2.301910	295.682041	4.421658
2.189278	285.189580	4.426662
2.214861	282.592773	4.431667
2.292104	291.202461	4.436672
2.390131	275.032671	4.441677
2.059067	275.925424	4.446682
2.139718	275.536380	4.451686
2.449636	280.583495	4.456691
2.100154	280.619501	4.461696
2.249706	280.655755	4.466701
2.045396	286.353984	4.471706
2.339660	287.315465	4.476710
2.506741	310.327925	4.481715
2.524796	312.743541	4.486720
3.117237	308.690054	4.491725
2.644586	305.836325	4.496730
2.464268	285.409876	4.501734
2.237251	286.204097	4.506739
2.603141	302.317882	4.511744
2.739164	312.306510	4.516749
2.845188	312.142965	4.521754
2.349789	293.903867	4.526758
2.574099	302.108743	4.531763
2.411880	305.710604	4.536768
2.985509	314.499384	4.541773
2.850200	319.511700	4.546778
2.743069	305.798757	4.551782
2.544867	303.518827	4.556787
2.671643	314.735832	4.561792
3.097718	301.659025	4.566797
2.656614	295.109279	4.571802
2.363509	285.144781	4.576806
2.647401	300.225072	4.581811
2.788055	312.784433	4.586816
3.043950	309.566353	4.591821
2.767716	316.541631	4.596826
3.105667	302.444579	4.601830
2.787373	315.304902	4.606835
2.596920	310.553025	4.611840
2.824130	303.500305	4.616845
2.437136	310.838076	4.621850
2.940074	312.964816	4.626854
2.923013	310.745665	4.631859
2.606821	314.988716	4.636864
3.074261	310.501854	4.641869
2.872190	316.960853	4.646874
2.802605	319.862026	4.651878
2.875446	317.565037	4.656883
2.785005	318.829987	4.661888
3.107242	304.255809	4.666893
2.745506	317.743755	4.671898
2.873395	311.614637	4.676902
2.933342	322.463432	4.681907
2.598408	311.641111	4.686912
2.620972	320.328740	4.691917
2.685733	327.078440	4.696922
3.260198	339.395884	4.701926
3.535066	343.543636	4.706931
2.916003	334.987606	4.711936
3.065828	331.735186	4.716941
3.144369	342.214065	4.721946
3.335849	330.815561	4.726950
3.136475	320.724024	4.731955
2.896203	327.219939	4.736960
3.209024	335.219943	4.741965
3.103470	349.477146	4.746970
3.248609	340.222291	4.751974
3.089315	352.173033	4.756979
2.992212	353.625377	4.761984
3.176116	339.963473	4.766989
2.947273	349.596159	4.771994
3.050117	350.735767	4.776998
3.430193	345.357384	4.782003
2.968515	348.246921	4.787008
3.171374	345.173582	4.792013
3.136110	349.121084	4.797018
3.305481	350.129496	4.802022
3.280050	341.095684	4.807027
3.336455	356.033530	4.812032
3.654961	341.359687	4.817037
3.456178	356.258485	4.822042
3.198233	350.862808	4.827046
3.280841	350.067120	4.832051
3.516390	349.552968	4.837056
3.915868	352.170653	4.842061
3.511350	359.212974	4.847066
3.589508	347.581616	4.852070
3.714896	353.872346	4.857075
3.158921	351.672174	4.862080
3.235461	349.523952	4.867085
3.319951	353.865246	4.872090
3.423774	343.294476	4.877094
3.467314	347.045602	4.882099
3.156130	354.884708	4.887104
3.155462	345.402389	4.892109
3.346579	353.408347	4.897114
3.252312	348.007274	4.902118
3.150631	364.703338	4.907123
3.438955	378.822134	4.912128
3.672064	375.296809	4.917133
3.886610	375.288161	4.922138
3.826900	372.813801	4.927142
3.766655	379.777812	4.932147
3.961313	370.596043	4.937152
3.638038	364.475305	4.942157
3.376348	369.866141	4.947162
3.938041	369.580768	4.952166
4.084469	373.075295	4.957171
3.468761	369.339855	4.962176
3.597388	357.619225	4.967181
3.520787	375.623640	4.972186
3.880828	369.285163	4.977190
3.825219	387.760912	4.982195
3.661046	380.259294	4.987200
4.250926	383.926277	4.992205
3.704147	376.738042	4.997210
3.914011	379.669718	5.002214
3.568315	369.172181	5.007219
3.699153	374.874147	5.012224
4.011914	376.576733	5.017229
3.537959	382.725768	5.022234
3.738359	374.111183	5.027238
3.550084	383.953653	5.032243
3.566419	382.265721	5.037248
3.830112	382.573162	5.042253
3.708824	386.793629	5.047258
3.828803	379.548070	5.052262
3.939337	378.944503	5.057267
3.810646	386.391489	5.062272
3.998481	393.299035	5.067277
3.568191	391.132708	5.072282
3.733795	387.302422	5.077286
4.089042	408.041517	5.082291
3.904528	408.669848	5.087296
3.949474	414.445253	5.092301
3.869919	425.739327	5.097306
4.464542	415.190644	5.102310
4.194169	418.076538	5.107315
3.981390	415.511087	5.112320
3.941122	411.381975	5.117325
4.086705	419.032404	5.122330
4.212980	410.557356	5.127334
4.341599	421.859976	5.132339
4.002033	417.411992	5.137344
4.145733	417.049604	5.142349
4.032213	421.324246	5.147354
4.285355	420.682658	5.152358
4.315138	420.349198	5.157363
4.567081	421.843406	5.162368
4.414268	415.985102	5.167373
4.235037	402.535421	5.172378
3.967474	391.258469	5.177382
4.059372	409.942678	5.182387
4.226924	417.542502	5.187392
4.152653	412.841411	5.192397
4.324063	419.389572	5.197402
4.365301	423.752255	5.202406
4.456858	418.664547	5.207411
4.317117	417.606903	5.212416
4.530130	414.171134	5.217421
4.186442	415.009546	5.222426
4.804098	415.584182	5.227430
4.318508	418.585635	5.232435
3.978926	419.914345	5.237440
4.294512	412.864110	5.242445
4.029604	428.562294	5.247450
4.354384	418.126373	5.252454
4.505956	423.734345	5.257459
4.170228	426.253751	5.262464
4.443854	419.502127	5.267469
4.002759	424.117548	5.272474
4.082469	422.918779	5.277478
4.378266	423.161308	5.282483
4.618760	439.447557	5.287488
4.710913	442.405445	5.292493
4.566430	440.862934	5.297498
4.239249	435.864489	5.302502
4.554595	440.363932	5.307507
4.751254	445.727245	5.312512
4.885059	445.976668	5.317517
4.485147	434.851843	5.322522
4.696351	429.043174	5.327526
4.402737	436.462831	5.332531
4.532300	451.128956	5.337536
5.286757	440.012291	5.342541
4.780685	436.015559	5.347546
4.606980	428.574697	5.352550
4.602773	426.373134	5.357555
4.680311	433.259099	5.362560
4.784996	426.498545	5.367565
4.516123	433.502059	5.372570
4.710283	442.971221	5.377574
4.813473	450.299327	5.382579
4.864195	450.839374	5.387584
5.034888	449.846360	5.392589
4.991462	448.903799	5.397594
4.907927	427.239214	5.402598
4.707578	423.735134	5.407603
4.432239	426.155936	5.412608
4.880347	448.411845	5.417613
4.882208	449.798870	5.422618
4.983147	456.702481	5.427622
5.173232	458.285871	5.432627
4.543067	440.656394	5.437632
4.484388	443.968617	5.442637
4.600012	459.302287	5.447642
4.874358	452.738791	5.452646
4.904408	446.249298	5.457651
4.641433	453.585743	5.462656
4.903475	448.088338	5.467661
4.707686	457.169976	5.472666
4.833211	455.583740	5.477670
4.930062	452.383679	5.482675
4.941262	464.866719	5.487680
4.995401	452.877734	5.492685
4.709739	461.351059	5.497690
5.310077	468.033252	5.502694
5.213049	470.648909	5.507699
5.005730	460.127607	5.512704
5.235931	456.856326	5.517709
4.796966	467.189503	5.522714
5.181061	468.511264	5.527718
5.329743	486.169077	5.532723
4.820889	486.066496	5.537728
5.234816	475.105851	5.542733
5.424917	488.809233	5.547738
5.420501	477.336298	5.552742
5.160023	465.547602	5.557747
4.750127	467.630152	5.562752
4.934118	470.456408	5.567757
4.932627	486.511040	5.572762
5.534006	487.462530	5.577766
5.257950	495.120849	5.582771
5.396350	483.935663	5.587776
5.711636	493.001764	5.592781
5.423852	494.143113	5.597786
5.343651	484.363858	5.602790
5.375632	487.094122	5.607795
5.480895	482.013990	5.612800
5.453428	481.497603	5.617805
5.491430	475.423956	5.622810
5.288629	464.129517	5.627814
5.388982	458.180533	5.632819
5.236751	474.767274	5.637824
5.171976	475.171140	5.642829
5.433460	492.892375	5.647834
5.421391	476.076163	5.652838
5.550550	479.851428	5.657843
5.358927	493.166905	5.662848
5.476112	487.599540	5.667853
5.234215	490.480139	5.672858
5.503928	479.753537	5.677862
5.502198	482.747107	5.682867
5.460180	480.310255	5.687872
5.475252	484.050538	5.692877
5.244662	492.171391	5.697882
5.282872	486.101455	5.702886
5.649434	487.145701	5.707891
5.573689	488.192145	5.712896
5.716034	486.368880	5.717901
5.386561	488.036727	5.722906
5.643291	486.755557	5.727910
5.436533	483.373691	5.732915
5.262771	490.079682	5.737920
5.406634	488.193213	5.742925
5.424312	499.810665	5.747930
5.697713	507.464048	5.752934
5.720957	512.885898	5.757939
5.650330	521.198339	5.762944
5.746051	513.958115	5.767949
5.619735	526.432993	5.772954
5.707030	518.856120	5.777958
5.490851	515.048764	5.782963
5.403144	517.281230	5.787968
5.701570	513.863857	5.792973
5.323584	513.295394	5.797978
5.408874	513.869977	5.802982
5.848130	511.832370	5.807987
5.666286	512.885729	5.812992
5.784980	522.929460	5.817997
5.382178	538.548563	5.823002
5.643740	533.462071	5.828006
6.218645	540.653499	5.833011
6.169040	540.443693	5.838016
6.548932	530.881076	5.843021
5.940395	525.854200	5.848026
5.534978	513.157431	5.853030
5.948950	530.573632	5.858035
6.086505	539.524144	5.863040
6.058702	533.126880	5.868045
5.929356	543.800362	5.873050
6.129206	537.940251	5.878054
6.109972	533.260202	5.883059
5.929410	532.050649	5.888064
6.107232	529.526670	5.893069
6.110251	531.715500	5.898074
6.051630	526.950410	5.903078
6.054855	518.921143	5.908083
6.085316	533.859312	5.913088
6.455495	532.622106	5.918093
6.020772	523.101239	5.923098
6.028896	510.845132	5.928102
6.042327	520.267502	5.933107
5.880427	539.999736	5.938112
6.236988	537.661851	5.943117
6.180499	540.533269	5.948122
6.065532	537.409508	5.953126
6.225930	538.594263	5.958131
6.026104	545.481409	5.963136
6.324388	536.208973	5.968141
6.263858	537.211854	5.973146
5.784370	541.828141	5.978150
6.037387	548.729897	5.983155
5.794257	547.404997	5.988160
6.045623	537.633954	5.993165
6.291613	550.388206	5.998170
6.299252	549.732996	6.003174
6.335908	546.657340	6.008179
5.952937	544.691546	6.013184
6.495672	540.866858	6.018189
6.336085	545.267960	6.023194
6.100493	549.779925	6.028198
6.407965	564.934914	6.033203
6.452581	576.324770	6.038208
6.549059	566.659081	6.043213
6.182421	563.594552	6.048218
6.413967	564.998416	6.053222
7.012739	556.805590	6.058227
6.383368	558.415947	6.063232
6.508205	541.895107	6.068237
6.531745	547.186873	6.073242
6.442628	537.814200	6.078246
6.393038	541.416410	6.083251
6.388077	535.882277	6.088256
6.304105	538.209640	6.093261
6.213824	544.981951	6.098266
6.246914	540.917423	6.103270
6.406204	538.028866	6.108275
5.973835	543.157539	6.113280
6.501037	538.898512	6.118285
6.389985	546.780157	6.123290
6.428593	542.345096	6.128294
6.253147	535.942283	6.133299
6.281659	551.277050	6.138304
6.380572	541.118807	6.143309
6.552342	542.651366	6.148314
6.308044	542.776518	6.153318
6.486312	545.648532	6.158323
6.215329	544.979862	6.163328
6.450062	540.915887	6.168333
6.286741	549.696982	6.173338
6.187169	546.897465	6.178342
6.414943	541.872214	6.183347
6.266326	540.837345	6.188352
6.228509	538.746711	6.193357
5.993966	545.503442	6.198362
6.500446	562.735240	6.203366
6.421802	569.451958	6.208371
6.352768	574.071725	6.213376
6.465418	569.944088	6.218381
6.216292	575.787587	6.223386
6.324738	568.441825	6.228390
6.932058	574.781312	6.233395
6.433350	562.176124	6.238400
6.603148	537.295216	6.243405
6.282777	543.065841	6.248410
6.423167	538.453885	6.253414
6.484836	539.344572	6.258419
6.261688	543.856250	6.263424
6.502363	534.624337	6.268429
6.431393	542.178467	6.273434
6.614177	538.846741	6.278438
6.482386	542.040650	6.283443
6.346242	550.230355	6.288448
6.778272	540.288691	6.293453
6.487221	543.180992	6.298458
6.623033	544.226549	6.303462
6.520837	541.568369	6.308467
6.413892	543.866975	6.313472
6.327021	536.843068	6.318477
6.344959	545.190586	6.323482
6.285652	541.144909	6.328486
6.745687	537.987901	6.333491
6.483108	544.717699	6.338496
6.717728	543.382760	6.343501
6.292561	522.576799	6.348506
6.466154	516.233417	6.353510
6.426011	515.109940	6.358515
6.122607	510.833151	6.363520
6.429479	515.393813	6.368525
6.268602	524.945496	6.373530
6.436157	528.070692	6.378534
6.017544	525.778679	6.383539
6.343030	537.608836	6.388544
6.552369	529.196537	6.393549
6.349409	539.552845	6.398554
6.403997	537.111236	6.403558
6.518833	537.342291	6.408563
6.630863	545.658836	6.413568
6.350905	522.475352	6.418573
6.457726	518.871447	6.423578
6.380095	509.033140	6.428582
6.249669	504.725540	6.433587
6.187827	511.551145	6.438592
6.457501	521.020086	6.443597
6.489889	522.493628	6.448602
6.064085	509.684794	6.453606
6.484462	510.687175	6.458611
6.335089	529.013643	6.463616
6.406208	527.731433	6.468621
6.442135	523.842269	6.473626
6.295670	519.868062	6.478630
6.520960	520.203967	6.483635
5.889644	523.485717	6.488640
6.328186	530.839635	6.493645
6.457231	535.745888	6.498650
6.215824	538.203713	6.503654
6.324541	529.488187	6.508659
6.361491	539.070072	6.513664
6.404810	530.373269	6.518669
6.334215	537.357811	6.523674
6.264443	536.385468	6.528678
6.404827	534.658429	6.533683
6.365739	544.080630	6.538688
6.301828	541.258436	6.543693
6.333272	540.966732	6.548698
6.342906	544.638664	6.553702
6.600987	535.239878	6.558707
6.412595	542.058429	6.563712
6.250076	537.161548	6.568717
6.617770	532.657395	6.573722
6.092997	539.733524	6.578726
6.602727	534.463260	6.583731
6.680187	543.705725	6.588736
6.646391	519.861835	6.593741
6.176330	519.781643	6.598746
6.094489	517.600816	6.603750
6.212534	523.195235	6.608755
6.588860	537.251650	6.613760
6.541982	536.105408	6.618765
6.270263	542.944072	6.623770
6.409023	531.533825	6.628774
6.582461	535.012076	6.633779
6.234042	524.157698	6.638784
6.729555	521.573814	6.643789
6.467653	514.814720	6.648794
6.479796	501.582899	6.653798
5.985854	504.448797	6.658803
6.137624	502.088982	6.663808
6.422538	509.877808	6.668813
6.439108	518.699154	6.673818
6.379494	509.046915	6.678822
6.602440	509.100618	6.683827
6.159417	514.391680	6.688832
6.311232	510.365322	6.693837
6.421334	515.530852	6.698842
6.436856	517.312472	6.703846
6.073747	514.972789	6.708851
6.082752	525.350231	6.713856
6.237479	532.252073	6.718861
6.254888	542.040259	6.723866
6.617494	544.286571	6.728870
6.677713	536.509925	6.733875
6.214302	540.733605	6.738880
6.444340	538.668872	6.743885
6.331587	538.582992	6.748890
6.249460	546.423734	6.753894
6.485511	539.723471	6.758899
6.458472	547.507335	6.763904
6.743653	536.357403	6.768909
6.015375	530.913443	6.773914
6.004527	534.937069	6.778918
6.364238	534.858997	6.783923
6.423319	538.073594	6.788928
6.736162	546.690787	6.793933
6.427512	540.454481	6.798938
6.387421	532.860213	6.803942
6.326593	524.726895	6.808947
6.286731	526.373036	6.813952
6.438569	533.817845	6.818957
6.407291	545.467907	6.823962
6.227833	528.205148	6.828966
6.473474	525.829193	6.833971
6.512282	535.472338	6.838976
6.539416	507.834975	6.843981
6.248878	513.785359	6.848986
5.619318	506.098477	6.853990
6.222925	526.368575	6.858995
6.236466	536.903540	6.864000
6.173484	529.477448	6.869005
6.334720	542.176461	6.874010
6.366814	540.259751	6.879014
6.665320	534.167218	6.884019
6.389547	532.127236	6.889024
6.597093	525.792634	6.894029
6.678580	533.727247	6.899034
6.615471	535.762052	6.904038
6.704325	527.422789	6.909043
6.388399	514.314744	6.914048
6.433765	503.154619	6.919053
6.360159	507.032337	6.924058
6.289199	499.870239	6.929062
6.383690	507.277762	6.934067
5.994980	509.533230	6.939072
6.738159	519.029144	6.944077
6.436997	516.468839	6.949082
6.455037	503.249656	6.954086
6.396217	510.928846	6.959091
6.227439	505.607744	6.964096
6.409706	497.626791	6.969101
6.293394	503.253891	6.974106
6.215464	503.456479	6.979110
6.452276	501.674205	6.984115
6.318155	506.160278	6.989120
6.477892	496.523626	6.994125
6.243052	516.514384	6.999130
6.328015	502.244535	7.004134
6.390426	501.371867	7.009139
6.475767	503.468126	7.014144
6.537177	495.163420	7.019149
6.856396	504.985674	7.024154
6.615507	506.975516	7.029158
6.684269	501.913854	7.034163
6.333821	511.390947	7.039168
6.332278	496.203984	7.044173
6.635422	512.805349	7.049178
6.289353	508.295857	7.054182
6.444325	506.836958	7.059187
6.151019	505.156476	7.064192
6.593650	505.677413	7.069197
6.577565	501.658138	7.074202
6.595536	499.728181	7.079206
6.741797	499.323927	7.084211
6.337278	507.315716	7.089216
6.930685	489.993303	7.094221
6.452022	478.336435	7.099226
6.309158	474.337567	7.104230
6.605756	476.887849	7.109235
6.044906	473.111725	7.114240
5.731767	473.358983	7.119245
6.111259	483.576182	7.124250
6.432929	498.950763	7.129254
6.625956	490.326677	7.134259
6.496411	503.539135	7.139264
6.482112	505.762009	7.144269
6.366682	504.298550	7.149274
6.322223	497.570160	7.154278
6.750626	493.762835	7.159283
6.276661	493.843726	7.164288
6.395319	472.624738	7.169293
6.208886	481.269905	7.174298
6.542484	476.334504	7.179302
6.234133	473.481559	7.184307
6.263471	477.020166	7.189312
6.156837	483.642022	7.194317
6.261172	493.391511	7.199322
6.483925	490.859901	7.204326
6.174585	495.257764	7.209331
6.365334	503.826673	7.214336
6.657377	502.731271	7.219341
6.525268	499.694621	7.224346
6.368040	496.048009	7.229350
6.413940	486.955729	7.234355
6.632680	482.836991	7.239360
6.485894	476.471292	7.244365
6.394252	483.387070	7.249370
6.086924	478.026758	7.254374
6.288454	479.208841	7.259379
6.145932	471.496386	7.264384
6.430841	486.003223	7.269389
6.395925	501.248392	7.274394
6.745035	493.903269	7.279398
6.487178	483.254156	7.284403
6.092877	477.362996	7.289408
6.306042	473.378981	7.294413
6.380749	472.093418	7.299418
6.222734	469.318591	7.304422
6.405018	472.497183	7.309427
6.259460	493.353656	7.314432
6.441284	493.074744	7.319437
6.343752	485.906791	7.324442
6.175404	489.520563	7.329446
6.380239	494.963844	7.334451
6.214924	501.972146	7.339456
6.363353	500.519067	7.344461
6.209617	503.726864	7.349466
6.316748	510.197496	7.354470
6.456290	501.118316	7.359475
6.189159	498.128099	7.364480
6.611316	498.032384	7.369485
6.396798	499.375518	7.374490
6.120482	499.117805	7.379494
6.668678	498.203376	7.384499
6.498336	496.848668	7.389504
6.456359	500.740881	7.394509
6.612524	506.422915	7.399514
6.109687	489.848785	7.404518
6.580620	496.702790	7.409523
6.495119	503.263335	7.414528
6.539457	483.434858	7.419533
6.575479	481.958756	7.424538
6.349836	477.148322	7.429542
6.383324	478.872299	7.434547
6.213974	480.809837	7.439552
6.099425	482.806186	7.444557
6.137674	489.461678	7.449562
6.551737	502.266995	7.454566
6.584395	498.218732	7.459571
6.360434	480.632259	7.464576
6.358196	483.117173	7.469581
6.257376	474.538201	7.474586
6.161335	484.924722	7.479590
6.462009	493.442270	7.484595
6.613742	495.611996	7.489600
6.629502	485.527748	7.494605
6.585912	481.317864	7.499610
6.106738	480.663936	7.504614
6.260494	474.335696	7.509619
6.242695	475.470030	7.514624
6.347099	478.723288	7.519629
6.411292	481.221868	7.524634
5.933982	479.982126	7.529638
6.487621	473.057224	7.534643
6.316124	496.142404	7.539648
6.658175	500.772028	7.544653
6.133237	499.149439	7.549658
6.182216	497.215927	7.554662
6.491932	496.188444	7.559667
6.508152	499.468542	7.564672
6.719640	502.500813	7.569677
6.137771	489.663964	7.574682
6.227835	480.449523	7.579686
6.162008	478.932070	7.584691
5.926313	498.621610	7.589696
6.515755	501.685033	7.594701
6.570302	506.336809	7.599706
6.498350	510.583871	7.604710
6.677904	498.725049	7.609715
6.286893	502.868056	7.614720
6.180839	490.076347	7.619725
6.538002	511.755784	7.624730
6.500881	504.453890	7.629734
6.275480	488.731519	7.634739
6.010743	491.383435	7.639744
6.530091	508.290787	7.644749
6.424345	503.660593	7.649754
6.366379	511.325434	7.654758
6.632779	497.631378	7.659763
6.361654	492.702962	7.664768
6.271100	484.549723	7.669773
6.186073	479.845458	7.674778
6.018838	495.196993	7.679782
6.372995	501.935555	7.684787
6.342367	504.930955	7.689792
6.033555	509.167113	7.694797
6.846390	513.793183	7.699802
6.377597	515.944496	7.704806
6.588705	510.604693	7.709811
6.363723	515.019773	7.714816
6.652643	508.429370	7.719821
6.417292	492.441642	7.724826
6.252262	481.123177	7.729830
6.514302	483.941445	7.734835
6.236955	502.821692	7.739840
6.447095	491.917867	7.744845
6.070710	490.200230	7.749850
6.117921	497.018427	7.754854
6.605802	505.996359	7.759859
6.625969	507.769907	7.764864
6.524592	494.282784	7.769869
6.285897	488.156280	7.774874
6.052194	490.126380	7.779878
6.190459	489.371989	7.784883
6.127756	514.440795	7.789888
6.107994	509.600798	7.794893
6.151825	513.231737	7.799898
6.049533	512.636173	7.804902
6.462091	509.824877	7.809907
6.086972	513.538607	7.814912
6.420008	507.538050	7.819917
6.751365	506.958693	7.824922
6.333529	509.241679	7.829926
6.633890	498.099917	7.834931
6.088101	511.771643	7.839936
6.480258	513.025767	7.844941
6.343671	508.785097	7.849946
6.532951	504.559143	7.854950
6.329439	505.525904	7.859955
6.058712	515.335144	7.864960
6.554359	497.527667	7.869965
6.119084	512.491232	7.874970
6.143279	516.791839	7.879974
6.367416	510.244921	7.884979
5.988053	516.555951	7.889984
6.180168	506.755862	7.894989
5.836816	518.265962	7.899994
5.888233	528.297748	7.904998
6.404097	530.671620	7.910003
6.401048	551.322230	7.915008
6.611231	545.146042	7.920013
6.578521	545.863700	7.925018
6.219462	541.223343	7.930022
6.477375	543.263404	7.935027
6.137204	553.149289	7.940032
6.291076	543.449444	7.945037
6.917095	544.465730	7.950042
7.004624	541.648652	7.955046
6.681662	530.252698	7.960051
6.263334	526.249700	7.965056
6.747278	508.916975	7.970061
6.495455	516.289097	7.975066
6.427521	517.964356	7.980070
6.396380	514.066961	7.985075
6.349261	518.719591	7.990080
5.984298	516.314698	7.995085
6.259863	513.979573	8.000090
6.221848	516.342540	8.005094
6.413211	514.073849	8.010099
6.276171	515.313379	8.015104
6.315667	513.367622	8.020109
6.088154	513.334983	8.025126
6.060495	515.769942	8.030144
6.249684	507.776429	8.035162
5.990112	521.471235	8.040179
6.389115	533.468530	8.045197
6.366147	542.820540	8.050214
6.498934	548.880062	8.055232
7.234546	536.668387	8.060250
6.770206	532.921961	8.065267
6.643532	517.389548	8.070285
6.558163	519.602781	8.075302
6.381711	517.013328	8.080320
6.399587	507.196149	8.085338
6.084103	520.496698	8.090355
6.394743	519.424900	8.095373
6.241778	514.402204	8.100390
6.077891	517.957281	8.105408
6.696093	512.138434	8.110426
6.389727	517.041024	8.115443
6.389759	518.002999	8.120461
6.447687	511.255148	8.125478
6.291112	516.800407	8.130496
6.429395	504.970520	8.135514
6.120955	517.159743	8.140531
6.656310	534.862402	8.145549
6.645970	544.207992	8.150566
6.479139	549.036113	8.155584
6.646580	537.653704	8.160602
6.263084	536.375608	8.165619
6.268508	537.455974	8.170637
6.040753	537.052224	8.175654
6.387317	548.491717	8.180672
6.282635	543.946809	8.185690
6.343556	555.933573	8.190707
6.383372	547.299268	8.195725
6.519527	550.488550	8.200742
6.501476	545.696241	8.205760
6.799550	545.816008	8.210778
6.421887	547.494221	8.215795
6.876796	549.379036	8.220813
6.788658	543.037024	8.225830
6.600718	554.983504	8.230848
6.815202	552.654880	8.235866
6.498190	555.198778	8.240883
6.672379	554.949715	8.245901
6.603626	550.794498	8.250918
6.512817	552.962774	8.255936
6.970611	547.606271	8.260954
6.898932	555.216280	8.265971
6.563419	549.453183	8.270989
7.024812	552.670494	8.276006
6.677602	556.978130	8.281024
6.746899	544.798637	8.286042
6.555093	554.633305	8.291059
6.629064	553.221981	8.296077
6.622763	553.899003	8.301094
6.693048	548.189766	8.306112
6.847323	543.050836	8.311130
6.484368	543.163533	8.316147
6.431339	549.611082	8.321165
6.638594	541.976543	8.326182
6.621323	543.015986	8.331200
6.695060	549.291964	8.336218
6.664696	553.594178	8.341235
6.381057	547.650456	8.346253
6.705713	543.831842	8.351270
6.381805	552.999651	8.356288
6.675387	540.161019	8.361306
6.606358	547.581819	8.366323
6.726157	541.124673	8.371341
6.690975	546.350650	8.376358
6.736988	550.004827	8.381376
6.840010	540.917570	8.386394
6.679771	539.581444	8.391411
6.719530	539.641629	8.396429
6.806950	542.080370	8.401446
6.727966	545.137766	8.406464
6.853830	543.517470	8.411482
6.613559	551.876013	8.416499
6.715550	554.231050	8.421517
6.473005	550.414235	8.426534
6.673441	552.474839	8.431552
6.660093	551.395865	8.436570
6.767868	548.175328	8.441587
6.924211	550.421765	8.446605
7.039215	549.317798	8.451622
6.847247	547.604077	8.456640
6.838774	544.875986	8.461658
7.132638	553.288397	8.466675
6.784135	552.541476	8.471693
6.880110	550.624771	8.476710
6.712607	546.269977	8.481728
6.906988	541.886164	8.486746
6.698440	543.935361	8.491763
6.586699	552.954858	8.496781
6.824438	548.542408	8.501798
6.742755	548.996496	8.506816
6.482906	555.458413	8.511834
6.806991	567.807881	8.516851
6.817272	576.511734	8.521869
7.217723	576.116747	8.526886
6.915243	586.287260	8.531904
6.991023	577.672572	8.536922
6.885695	581.118170	8.541939
6.808302	579.535070	8.546957
7.077261	582.009304	8.551974
6.867920	590.043082	8.556992
7.120098	584.473584	8.562010
6.898569	571.126757	8.567027
7.050895	573.084511	8.572045
7.056428	554.874049	8.577063
6.663618	553.680952	8.582080
6.674003	554.576062	8.587098
7.207589	579.742530	8.592115
7.367264	580.447578	8.597133
7.121769	555.598028	8.602151
6.751075	556.917829	8.607168
6.751398	555.844268	8.612186
7.205046	571.435053	8.617203
7.018677	579.726028	8.622221
7.240611	562.284591	8.627239
6.976745	551.562133	8.632256
7.061825	556.271776	8.637274
7.089475	548.858300	8.642291
7.007017	554.949135	8.647309
6.967282	540.297320	8.652327
6.862768	553.985375	8.657344
6.804200	557.668090	8.662362
6.893961	574.729273	8.667379
6.689253	573.511326	8.672397
7.287085	579.114943	8.677415
7.168913	579.070383	8.682432
7.337835	584.252931	8.687450
7.424361	571.151137	8.692467
6.843901	566.110044	8.697485
7.453952	563.083283	8.702503
7.148284	565.970360	8.707520
6.995676	547.016263	8.712538
6.973401	552.130663	8.717555
7.078150	571.027029	8.722573
6.819899	561.999189	8.727591
6.810969	573.033424	8.732608
6.782276	577.354067	8.737626
7.049649	578.407005	8.742643
6.676394	578.506645	8.747661
6.863001	573.149372	8.752679
7.102434	579.240063	8.757696
7.122017	573.849428	8.762714
7.143010	580.985670	8.767731
7.212801	573.476233	8.772749
7.182800	584.560026	8.777767
7.131766	586.707941	8.782784
7.039213	585.781048	8.787802
7.076402	580.490638	8.792819
6.805076	576.929156	8.797837
7.234516	585.845674	8.802855
7.366823	594.546456	8.807872
7.252268	599.541122	8.812890
7.489907	600.062406	8.817907
7.760224	586.136715	8.822925
7.432015	578.228643	8.827943
7.233958	579.684809	8.832960
7.078405	575.393181	8.837978
7.428319	575.066204	8.842995
7.362008	584.424433	8.848013
7.395909	574.234504	8.853031
7.350115	578.644194	8.858048
7.493099	578.180627	8.863066
7.611445	572.333117	8.868083
7.178207	579.477255	8.873101
7.455831	572.967980	8.878119
7.311916	574.633080	8.883136
7.285454	577.166072	8.888154
7.243948	576.034873	8.893171
7.199995	583.393667	8.898189
7.195588	578.331391	8.903207
7.325179	582.858881	8.908224
7.104160	585.634116	8.913242
7.309102	567.161108	8.918259
7.175822	577.256947	8.923277
7.140749	574.348424	8.928295
7.364622	572.139494	8.933312
7.448143	571.559601	8.938330
7.381449	575.122415	8.943347
7.157363	580.312561	8.948365
7.451102	574.251965	8.953383
7.137731	570.003006	8.958400
7.244871	571.250180	8.963418
7.434856	582.133973	8.968435
7.797066	597.287003	8.973453
7.753954	592.851563	8.978471
7.678930	577.159169	8.983488
7.388288	581.504685	8.988506
7.209469	578.356596	8.993523
7.218824	573.162130	8.998541
7.637094	579.240726	9.003559
7.745397	576.496048	9.008576
7.395314	581.967671	9.013594
7.442125	567.199341	9.018611
7.344625	580.779179	9.023629
7.319075	581.931798	9.028647
7.673914	572.231211	9.033664
7.451307	575.817873	9.038682
7.543547	571.590326	9.043699
7.172864	570.659491	9.048717
7.254925	575.161977	9.053735
7.613950	588.125713	9.058752
7.521410	594.510340	9.063770
7.713251	591.106003	9.068787
7.393658	586.082529	9.073805
7.327665	585.077030	9.078823
7.500163	591.535281	9.083840
7.549108	616.886974	9.088858
7.863414	606.122084	9.093875
7.535145	594.161129	9.098893
7.617721	586.087599	9.103911
7.505277	590.432742	9.108928
7.412504	592.069101	9.113946
7.756606	600.550576	9.118963
7.644083	610.752638	9.123981
7.508091	609.017831	9.128999
7.677587	604.725321	9.134016
7.526928	604.494223	9.139034
7.625059	601.541002	9.144051
7.445361	598.449744	9.149069
7.506273	609.174232	9.154087
7.487124	615.929367	9.159104
7.584847	615.189257	9.164122
7.773605	612.949524	9.169139
7.587562	614.371226	9.174157
7.546356	610.873593	9.179175
7.614618	608.868759	9.184192
7.479885	610.964597	9.189210
7.759116	615.091752	9.194227
7.668366	617.169285	9.199245
7.608092	619.291768	9.204263
8.290460	609.660144	9.209280
7.779061	613.139132	9.214298
8.002465	603.354391	9.219315
7.981482	616.074007	9.224333
7.753260	607.447441	9.229351
7.748147	581.141406	9.234368
7.676733	599.186524	9.239386
7.981914	596.509826	9.244403
7.731901	587.430216	9.249421
7.296350	584.372272	9.254439
7.725735	595.287294	9.259456
7.911742	605.823360	9.264474
7.947711	610.988958	9.269491
7.486996	604.617085	9.274509
8.043826	609.233080	9.279527
8.028825	610.020199	9.284544
7.700778	614.617178	9.289562
7.731003	602.347856	9.294579
7.965455	618.855046	9.299597
7.937950	615.637802	9.304615
7.849595	589.540406	9.309632
7.520809	593.664501	9.314650
7.737216	608.505487	9.319667
7.934683	615.384585	9.324685
7.681222	610.573368	9.329703
7.835579	620.611371	9.334720
7.959794	623.721350	9.339738
7.990152	613.161927	9.344755
7.884421	608.930540	9.349773
7.692064	611.310704	9.354791
8.042659	608.041877	9.359808
7.886384	612.812368	9.364826
7.979230	605.436884	9.369843
7.721199	610.417124	9.374861
7.782311	617.970729	9.379879
7.866053	611.319144	9.384896
7.965056	624.897583	9.389914
7.848764	610.208775	9.394931
7.643780	608.769626	9.399949
7.960792	613.669608	9.404967
8.021447	603.745881	9.409984
7.673952	613.901820	9.415002
8.054888	607.375817	9.420019
7.796076	605.571787	9.425037
7.698403	615.587547	9.430055
8.038525	607.148349	9.435072
7.607336	615.649950	9.440090
7.544342	612.012626	9.445107
8.035834	619.676451	9.450125
7.962004	629.906959	9.455143
8.265177	632.504267	9.460160
7.946864	632.552292	9.465178
7.790647	628.946936	9.470195
8.123966	641.653966	9.475213
8.274489	638.056079	9.480231
8.364934	624.754982	9.485248
7.883110	628.051530	9.490266
7.952907	618.620539	9.495283
7.959359	616.869231	9.500301
8.278953	631.563830	9.505319
8.574578	629.979191	9.510336
7.969299	628.746865	9.515354
8.101921	607.326328	9.520371
7.947247	606.482942	9.525389
7.890199	613.281161	9.530407
8.224114	621.578913	9.535424
8.238591	632.849851	9.540442
8.409960	625.400336	9.545459
8.176520	617.347820	9.550477
8.003794	624.731106	9.555495
8.176364	615.142558	9.560512
7.779318	615.582729	9.565530
8.005888	627.458266	9.570547
8.126466	629.703944	9.575565
8.097306	627.080635	9.580583
8.101203	632.069082	9.585600
7.866941	634.187308	9.590618
8.051451	626.591138	9.595635
8.328917	623.193480	9.600653
8.079956	633.239224	9.605671
8.093628	625.328057	9.610688
7.934353	629.862057	9.615706
7.991467	628.810975	9.620723
8.081523	627.255258	9.625741
8.176750	626.791527	9.630759
8.183511	622.339159	9.635776
8.141386	629.796879	9.640794
8.397819	641.372619	9.645811
8.402545	631.716190	9.650829
8.027051	637.752437	9.655847
8.384900	640.707206	9.660864
8.567052	663.461096	9.665882
8.436607	637.382399	9.670899
8.344547	641.762762	9.675917
7.810551	633.258856	9.680935
8.407615	645.770258	9.685952
8.380776	660.988756	9.690970
8.475243	656.575789	9.695987
8.780250	643.326937	9.701005
8.275991	643.317569	9.706023
8.490882	633.998362	9.711040
8.258822	638.199557	9.716058
8.121408	628.737521	9.721075
8.415235	636.571084	9.726093
8.442913	649.834998	9.731111
8.838224	640.977613	9.736128
8.542164	635.997861	9.741146
8.399406	631.444273	9.746163
8.677364	632.400980	9.751181
8.057936	628.061746	9.756199
8.366809	623.298346	9.761216
8.140467	630.948764	9.766234
8.347399	632.414444	9.771251
8.383570	645.880479	9.776269
8.369782	661.087367	9.781287
8.990682	653.106344	9.786304
8.675961	651.536159	9.791322
8.544978	638.385881	9.796339
8.812795	632.395102	9.801357
8.465141	633.543979	9.806375
8.978488	633.281075	9.811392
8.469549	632.712281	9.816410
8.487978	627.157656	9.821427
8.817304	629.021546	9.826445
8.324419	633.454499	9.831463
8.566903	633.331322	9.836480
8.579339	628.250888	9.841498
8.377262	632.287677	9.846515
8.481152	623.798222	9.851533
8.578478	621.748420	9.856551
8.627165	623.583587	9.861568
8.995357	628.719966	9.866586
8.402997	626.080866	9.871603
8.694533	616.028552	9.876621
8.544588	627.145622	9.881639
8.558814	623.177813	9.886656
8.567096	618.972029	9.891674
8.379799	624.842078	9.896691
8.521098	625.656463	9.901709
8.032436	629.750155	9.906727
8.683174	645.731188	9.911744
8.768923	652.615023	9.916762
8.797158	659.936311	9.921779
8.725012	653.588457	9.926797
8.715630	654.151434	9.931815
8.780006	641.777022	9.936832
8.658443	643.999416	9.941850
8.790209	650.015448	9.946867
8.759722	638.883836	9.951885
8.363308	641.870986	9.956903
8.633880	639.036243	9.961920
8.517708	643.928835	9.966938
8.612270	654.991658	9.971955
8.478896	657.896282	9.976973
8.778904	663.378981	9.981991
8.943794	654.271966	9.987008
8.987500	657.597633	9.992026
8.814143	661.470629	9.997043
9.277092	657.240726	10.002061
8.513087	667.301702	10.007079
8.771365	657.594217	10.012096
8.930654	657.610399	10.017114
8.684720	654.779688	10.022131
8.816966	655.924293	10.027149
8.768854	658.746299	10.032167
8.896989	661.337953	10.037184
8.894895	652.451885	10.042202
9.077330	654.058229	10.047219
9.009835	654.369821	10.052237
8.661448	660.455916	10.057255
8.749299	653.316261	10.062272
9.069473	665.859750	10.067290
8.805397	661.509301	10.072307
8.835501	655.478352	10.077325
8.589060	662.341612	10.082343
8.601766	665.138983	10.087360
8.902687	653.938311	10.092378
8.808321	666.274081	10.097395
9.219058	658.591225	10.102413
9.090045	662.218705	10.107431
8.947982	661.711593	10.112448
8.925672	652.854067	10.117466
9.178695	658.759479	10.122483
9.185790	655.075896	10.127501
8.932188	661.631700	10.132519
8.998092	654.594492	10.137536
9.071850	653.507583	10.142554
9.075924	658.863703	10.147571
9.365788	656.766267	10.152589
8.795931	670.077570	10.157607
8.770676	665.680488	10.162624
8.760304	659.455465	10.167642
8.882813	664.832918	10.172659
9.120325	652.800672	10.177677
8.905410	655.568020	10.182695
8.918588	657.331910	10.187712
8.931127	667.396183	10.192730
8.876302	665.087728	10.197747
9.074195	660.804475	10.202765
9.038861	666.579696	10.207783
9.140680	657.721297	10.212800
9.395813	656.285870	10.217818
9.067555	664.068134	10.222835
9.574417	661.201740	10.227853
9.214200	652.056881	10.232871
8.977684	662.052161	10.237888
9.448936	657.992526	10.242906
9.112346	660.228481	10.247923
9.398837	654.633395	10.252941
9.289550	662.164059	10.257959
9.320556	653.172909	10.262976
9.072357	655.685154	10.267994
8.971666	662.941970	10.273011
9.329045	658.961817	10.278029
9.273209	653.084461	10.283047
9.200496	652.059205	10.288064
9.090222	648.014768	10.293082
9.163710	661.043954	10.298099
9.066381	654.280611	10.303117
9.038175	651.487071	10.308135
9.087053	654.626460	10.313152
9.006284	660.069459	10.318170
9.225215	675.870466	10.323187
9.363739	680.892144	10.328205
9.831716	682.114223	10.333223
9.059415	670.314918	10.338240
9.254827	655.446509	10.343258
9.619109	662.683809	10.348275
9.464241	653.845082	10.353293
9.469188	658.198364	10.358311
9.447412	646.298816	10.363328
9.200549	654.437653	10.368346
8.878052	654.448972	10.373363
9.101647	662.544949	10.378381
9.081819	666.183088	10.383399
8.988151	672.043950	10.388416
9.751320	676.429157	10.393434
9.571004	683.833018	10.398451
9.516113	679.712083	10.403469
9.597876	686.260393	10.408487
9.698029	681.202816	10.413504
9.778260	665.208263	10.418522
9.454415	657.376982	10.423539
9.498624	652.608975	10.428557
9.450958	653.797150	10.433575
9.575786	651.199516	10.438592
9.544142	647.877839	10.443610
9.518827	653.134893	10.448627
9.520290	649.060143	10.453645
9.330331	652.586302	10.458663
9.270107	652.082174	10.463680
9.665429	643.849156	10.468698
9.165565	658.853083	10.473715
9.555822	660.842313	10.478733
9.889026	675.004024	10.483751
9.626830	667.164892	10.488768
9.792319	654.918994	10.493786
9.442293	659.661349	10.498803
9.398407	646.834417	10.503821
9.296898	660.112645	10.508839
9.503654	671.090764	10.513856
9.744891	677.641403	10.518874
9.507101	685.739780	10.523891
9.594772	682.061745	10.528909
9.598859	683.573222	10.533927
9.574539	679.674377	10.538944
9.943197	683.469833	10.543962
9.598567	680.035024	10.548979
9.538480	678.685254	10.553997
9.650302	676.667688	10.559015
9.562708	681.613430	10.564032
9.815977	682.365580	10.569050
9.810769	690.948644	10.574067
9.792430	682.767174	10.579085
9.793712	678.965657	10.584103
9.485368	680.800112	10.589120
10.159706	677.928030	10.594138
9.672659	679.248013	10.599155
9.792954	660.886738	10.604173
9.845664	657.263708	10.609191
9.777453	650.691201	10.614208
9.959171	652.427971	10.619226
9.477606	647.355712	10.624243
9.516196	655.883082	10.629261
9.900369	671.553972	10.634279
9.924280	681.602199	10.639296
10.253459	664.565697	10.644314
9.538657	657.450688	10.649331
9.682141	651.450964	10.654349
9.926851	662.940084	10.659367
9.863892	675.186807	10.664384
9.848664	671.856502	10.669402
9.850702	674.879249	10.674419
9.726349	680.690081	10.679437
9.868448	677.744722	10.684455
9.962377	677.335926	10.689472
10.068368	680.966227	10.694490
9.683557	680.713470	10.699507
9.791379	675.512507	10.704525
10.031023	683.838895	10.709543
10.116923	686.989482	10.714560
10.399081	675.849378	10.719578
9.772584	656.070521	10.724595
9.684345	651.154378	10.729613
10.022497	661.324956	10.734631
9.900795	673.002307	10.739648
10.209971	668.421902	10.744666
9.984737	668.014778	10.749683
10.077720	664.896069	10.754701
9.606951	668.010490	10.759719
9.687009	672.361968	10.764736
9.981958	671.804933	10.769754
9.695719	679.992820	10.774771
9.981166	678.213023	10.779789
9.758079	677.423282	10.784807
9.559590	679.846596	10.789824
9.853525	687.840000	10.794842
10.088433	684.535592	10.799859
9.584432	677.753361	10.804877
9.999713	689.326848	10.809895
10.218553	702.080048	10.814912
10.385075	698.472019	10.819930
9.866740	693.962493	10.824947
10.210880	694.742113	10.829965
10.088473	697.285501	10.834983
9.896657	699.799046	10.840000
10.286724	703.992907	10.845018
10.313668	711.995102	10.850035
10.059473	714.026881	10.855053
10.186128	714.718113	10.860071
10.391684	715.084880	10.865088
10.296598	705.559493	10.870106
10.112200	699.384529	10.875123
9.981951	708.390646	10.880141
10.356716	704.846946	10.885159
10.112270	715.378187	10.890176
10.623328	705.521342	10.895194
10.856174	701.517313	10.900211
10.152291	692.837579	10.905229
10.229832	677.731201	10.910247
10.459934	677.884467	10.915264
10.353597	673.612220	10.920282
10.282461	675.296379	10.925299
10.375612	670.328935	10.930317
10.262397	673.607759	10.935335
10.211601	680.814199	10.940352
10.365622	674.469435	10.945370
10.077979	672.352277	10.950387
9.990717	677.112541	10.955405
10.451771	683.408293	10.960423
10.532240	694.467967	10.965440
10.706071	679.467289	10.970458
10.400135	686.576224	10.975475
10.483030	679.934592	10.980493
10.364348	666.951928	10.985511
10.163940	675.151583	10.990528
10.495395	668.374709	10.995546
10.493551	674.410120	11.000563
10.254954	684.049874	11.005581
10.507136	675.611422	11.010599
10.399278	685.757056	11.015616
10.318320	686.703517	11.020634
10.413441	700.427931	11.025651
10.462296	702.326856	11.030669
11.150465	701.137813	11.035687
10.408992	688.842867	11.040704
10.492038	671.771134	11.045722
10.606972	675.558998	11.050739
10.109870	676.172422	11.055757
10.724175	688.394407	11.060775
10.625035	698.719304	11.065792
10.556521	702.487554	11.070810
10.821180	698.416450	11.075827
10.696845	683.478526	11.080845
11.271661	666.915490	11.085863
10.577030	679.280198	11.090880
10.384093	669.145877	11.095898
10.545096	672.306071	11.100915
10.240804	667.043437	11.105933
10.406388	667.724678	11.110951
10.418475	682.936752	11.115968
10.682278	690.043861	11.120986
10.664457	700.843060	11.126003
10.843297	700.248167	11.131021
10.472725	696.906621	11.136039
10.601904	709.395163	11.141056
10.612958	708.957178	11.146074
10.616761	697.831262	11.151091
10.575105	706.489264	11.156109
10.921302	704.473827	11.161127
10.751336	707.669935	11.166144
10.635401	705.825503	11.171162
10.824801	705.169416	11.176179
10.433616	710.427627	11.181197
11.117629	703.740382	11.186215
10.824949	712.121074	11.191232
10.598603	701.603310	11.196250
10.688600	701.733322	11.201267
10.392770	701.180415	11.206285
10.815575	696.256796	11.211303
10.592417	702.266269	11.216320
11.005479	704.454079	11.221338
10.918108	695.990349	11.226355
10.689120	709.558216	11.231373
10.944710	709.028168	11.236391
10.692589	710.467906	11.241408
10.613862	706.121003	11.246426
10.704451	701.209482	11.251443
10.868268	714.451302	11.256461
10.837257	700.605324	11.261479
10.579539	710.525016	11.266496
11.139912	712.019969	11.271514
11.401489	722.183583	11.276531
11.348256	715.229851	11.281549
11.035279	702.722611	11.286567
11.162065	706.085710	11.291584
11.128507	704.705562	11.296602
11.400533	707.325757	11.301619
10.709303	705.291563	11.306637
10.886519	699.825179	11.311655
10.925460	706.865206	11.316672
10.894514	694.514016	11.321690
11.270854	698.470399	11.326707
11.144578	705.918863	11.331725
11.261739	701.550154	11.336743
10.901457	707.481159	11.341760
10.765425	698.153096	11.346778
11.290244	698.689426	11.351795
11.133762	704.406774	11.356813
11.282360	697.673551	11.361831
10.878588	710.207037	11.366848
10.893145	702.868485	11.371866
11.121549	699.538381	11.376883
10.786574	712.073862	11.381901
11.171111	702.014754	11.386919
10.900045	708.568351	11.391936
11.056591	715.294831	11.396954
11.401175	718.912009	11.401971
11.243895	726.475059	11.406989
11.459967	737.688284	11.412007
11.007970	714.267672	11.417024
11.340197	724.812480	11.422042
11.814396	720.440547	11.427059
11.162483	708.562227	11.432077
11.129330	695.729540	11.437095
10.947131	703.116007	11.442112
10.557532	714.258649	11.447130
11.213815	723.128238	11.452147
11.366346	741.356702	11.457165
11.502502	732.436278	11.462183
11.444420	743.349648	11.467200
11.374642	737.556847	11.472218
11.713169	731.863753	11.477235
11.567418	733.753175	11.482253
11.399721	718.847198	11.487271
11.467630	717.698265	11.492288
11.273343	702.276659	11.497306
11.366255	697.673004	11.502323
11.363583	722.495654	11.507341
11.334921	721.985904	11.512359
11.546646	733.409282	11.517376
11.426803	726.646092	11.522394
11.311922	711.728620	11.527411
11.476000	718.519205	11.532429
11.455738	724.408874	11.537447
11.354158	720.260228	11.542464
11.507646	727.474986	11.547482
11.635785	724.326037	11.552499
11.354942	730.072647	11.557517
11.688520	726.139328	11.562535
11.154209	733.078631	11.567552
11.193846	728.543628	11.572570
11.523808	725.626204	11.577587
11.560216	727.896857	11.582605
11.697041	725.932227	11.587623
11.478402	721.904533	11.592640
11.441219	722.510696	11.597658
11.640945	721.193094	11.602675
11.424659	721.251388	11.607693
11.698820	725.738447	11.612711
11.502479	730.005401	11.617728
11.180620	727.766349	11.622746
11.468927	722.613827	11.627763
11.344047	726.352048	11.632781
11.449926	729.834355	11.637799
11.755614	739.470234	11.642816
11.542569	730.154904	11.647834
11.466672	738.733165	11.652851
11.804701	752.920919	11.657869
12.178806	745.602728	11.662887
11.992817	734.184215	11.667904
11.904606	723.485304	11.672922
11.696024	720.158266	11.677939
11.753554	718.159526	11.682957
12.110346	714.120404	11.687975
11.962879	721.798356	11.692992
12.090712	722.301215	11.698010
12.079208	717.789249	11.703027
11.917994	722.068887	11.708045
12.011632	717.957597	11.713063
12.205814	727.910734	11.718080
11.893422	727.264905	11.723098
12.120289	713.514395	11.728115
11.795037	727.891872	11.733133
12.065648	718.949980	11.738151
12.348146	714.949142	11.743168
11.983078	703.265047	11.748186
12.111595	692.849542	11.753203
11.863155	689.027173	11.758221
11.603518	689.737882	11.763239
12.031123	687.109003	11.768256
11.938584	698.588643	11.773274
11.944329	684.199617	11.778291
11.832689	693.060920	11.783309
12.053112	690.030940	11.788327
11.783707	707.454481	11.793344
11.706313	710.968706	11.798362
12.294766	722.521811	11.803379
11.936358	719.234148	11.808397
12.203796	716.695562	11.813415
12.174087	720.640057	11.818432
11.596417	711.347322	11.823450
12.053257	710.645769	11.828467
11.984779	717.864996	11.833485
11.967323	719.502478	11.838503
11.909009	718.335078	11.843520
11.787568	715.269974	11.848538
12.267889	711.824535	11.853555
12.359550	715.810346	11.858573
12.047337	723.501011	11.863591
12.284425	709.885419	11.868608
11.876694	716.299847	11.873626
11.897570	723.613329	11.878643
11.965274	717.993823	11.883661
11.897314	716.459931	11.888679
12.253548	723.785202	11.893696
11.751483	722.986539	11.898714
12.320788	715.735640	11.903731
12.140298	720.211765	11.908749
12.289270	734.908733	11.913767
12.551181	725.760809	11.918784
12.399639	723.036101	11.923802
12.290616	726.337076	11.928819
12.302530	723.641599	11.933837
11.982258	722.183342	11.938855
12.275642	706.152271	11.943872
12.093570	723.226741	11.948890
12.517321	739.189949	11.953907
12.489394	747.129993	11.958925
12.176750	731.244518	11.963943
12.345889	728.136807	11.968960
12.330403	743.366498	11.973978
12.725882	736.817562	11.978995
12.647070	735.786224	11.984013
12.391117	722.306589	11.989031
12.374160	718.406907	11.994048
12.231443	714.422939	11.999066
12.363099	720.610661	12.004083
12.287222	742.546814	12.009101
12.222202	740.700640	12.014119
12.704546	738.656750	12.019136
12.676767	748.603349	12.024154
12.804965	744.409562	12.029171
12.787126	738.658158	12.034189
12.840215	728.724384	12.039207
12.647391	712.040393	12.044224
12.315223	715.216907	12.049242
12.367099	706.803338	12.054259
12.760378	714.744482	12.059277
12.467807	712.755292	12.064295
12.555565	703.209865	12.069312
12.432836	706.238712	12.074330
12.700187	729.014810	12.079347
12.878140	728.492106	12.084365
12.749729	722.915701	12.089383
12.298841	712.155205	12.094400
12.397371	721.352568	12.099418
12.698279	735.045300	12.104435
12.478526	739.398412	12.109453
12.774534	738.519958	12.114471
12.797433	734.162518	12.119488
12.606518	738.813594	12.124506
12.499701	740.047394	12.129523
12.856084	739.181383	12.134541
12.758423	741.204961	12.139559
12.910872	740.115252	12.144576
12.799783	738.258991	12.149594
12.929171	745.012814	12.154611
13.014260	737.281092	12.159629
12.674043	736.394608	12.164647
12.912769	730.497973	12.169664
12.513172	739.888453	12.174682
12.539544	738.875129	12.179699
12.932674	730.467242	12.184717
12.842720	741.215818	12.189735
12.809468	733.316303	12.194752
12.623762	743.463448	12.199770
12.878231	727.421871	12.204787
13.086945	723.008076	12.209805
12.939093	741.787039	12.214823
13.118609	740.170436	12.219840
12.829321	737.988584	12.224858
12.559244	739.213987	12.229875
12.769782	737.137550	12.234893
12.816345	740.279308	12.239911
13.048425	735.208135	12.244928
12.875187	744.635147	12.249946
12.941107	745.862786	12.254963
13.207872	732.868601	12.259981
12.709215	742.203836	12.264999
12.753496	739.558111	12.270016
13.082470	752.805686	12.275034
13.290208	753.377987	12.280051
13.270126	744.012588	12.285069
12.702694	740.241451	12.290087
13.246321	750.222955	12.295104
13.200002	763.714955	12.300122
13.261284	750.293783	12.305139
13.325111	738.753984	12.310157
12.860941	734.089422	12.315175
13.319488	742.919328	12.320192
12.957078	743.779726	12.325210
13.007885	753.562144	12.330227
13.617760	751.471939	12.335245
13.304883	748.687332	12.340263
13.495283	735.364078	12.345280
13.199693	737.309412	12.350298
13.039088	722.174712	12.355315
13.207171	732.780955	12.360333
13.405586	746.523344	12.365351
13.549126	752.238665	12.370368
13.270726	742.801873	12.375386
13.196925	741.190998	12.380403
13.413158	731.123127	12.385421
13.360572	731.157858	12.390439
13.371948	724.814647	12.395456
13.236646	733.822797	12.400474
13.178719	736.212215	12.405491
13.885418	740.115481	12.410509
13.113191	746.027317	12.415527
13.563018	734.918852	12.420544
13.358264	739.496240	12.425562
13.458355	748.562265	12.430579
13.585832	739.404705	12.435597
13.275883	728.359458	12.440615
13.569776	736.107633	12.445632
13.377477	745.722044	12.450650
13.396225	750.523435	12.455667
13.907766	748.556200	12.460685
13.290279	755.591171	12.465703
13.566610	738.624753	12.470720
13.742221	749.620290	12.475738
13.367474	752.914093	12.480755
13.693353	752.364925	12.485773
13.474656	752.565736	12.490791
13.578145	737.994343	12.495808
13.648370	758.520578	12.500826
13.721136	764.996401	12.505843
13.752276	744.646356	12.510861
13.229612	744.767979	12.515879
13.628185	747.880190	12.520896
13.789671	759.556381	12.525914
13.732219	761.864627	12.530931
13.797355	755.354636	12.535949
13.530326	762.799270	12.540967
13.616101	764.227942	12.545984
13.657008	760.637942	12.551002
13.600466	756.466869	12.556019
13.602092	761.706901	12.561037
13.795068	756.275287	12.566055
13.910952	759.583907	12.571072
13.941664	757.733689	12.576090
13.493445	761.413260	12.581107
13.966052	755.955815	12.586125
13.836308	762.279746	12.591143
14.103830	757.067272	12.596160
14.162808	761.482498	12.601178
13.821070	769.591832	12.606195
14.010795	758.884274	12.611213
13.795664	764.201141	12.616231
13.695113	757.854011	12.621248
14.249767	761.971425	12.626266
13.675141	762.720516	12.631283
13.809037	762.964906	12.636301
13.789383	760.919889	12.641319
14.202118	752.775658	12.646336
14.096061	756.363534	12.651354
14.235046	759.735648	12.656371
14.305943	757.887437	12.661389
13.756402	762.386891	12.666407
14.027750	752.015409	12.671424
13.888884	757.814893	12.676442
14.088295	760.485308	12.681459
14.131744	756.232721	12.686477
13.727670	759.969152	12.691495
13.770855	754.202519	12.696512
13.904954	761.152015	12.701530
13.732215	757.388743	12.706547
14.047527	754.679634	12.711565
13.967361	756.335771	12.716583
13.673698	750.897736	12.721600
14.138867	768.824873	12.726618
14.300764	778.924326	12.731635
14.687830	773.971170	12.736653
14.420716	753.808287	12.741671
14.207491	757.194235	12.746688
14.312201	760.218108	12.751706
13.923781	745.016782	12.756723
14.157902	743.550184	12.761741
14.075356	752.319700	12.766759
14.362211	764.675097	12.771776
14.837750	767.850154	12.776794
14.203885	765.905266	12.781811
14.102728	753.780210	12.786829
13.993943	764.052026	12.791847
14.419773	768.265178	12.796864
14.866327	771.364725	12.801882
14.051092	767.838933	12.806899
14.186366	769.501915	12.811917
14.295930	784.617638	12.816935
14.480391	784.437536	12.821952
14.468894	782.466752	12.826970
14.676900	791.878694	12.831987
14.577555	776.052337	12.837005
14.318785	768.111410	12.842023
14.516385	784.366036	12.847040
14.735216	774.189839	12.852058
14.520135	761.895855	12.857075
14.416781	752.143080	12.862093
14.449107	762.831663	12.867111
14.487795	766.747916	12.872128
14.735716	779.440069	12.877146
14.322068	775.365127	12.882163
14.374660	778.935793	12.887181
14.292894	782.379896	12.892199
14.384996	786.018033	12.897216
14.483729	775.465286	12.902234
14.428849	785.351046	12.907251
14.702038	779.523092	12.912269
14.527698	781.052313	12.917287
14.324253	776.631558	12.922304
14.803652	776.826612	12.927322
14.520512	787.319823	12.932339
14.810234	773.976152	12.937357
14.559703	773.952326	12.942375
14.503698	769.604005	12.947392
14.801025	774.702563	12.952410
14.713062	785.620517	12.957427
14.693158	780.128874	12.962445
15.041884	798.203665	12.967463
14.985363	794.636089	12.972480
15.278959	775.421617	12.977498
15.061594	769.139097	12.982515
14.985147	766.116923	12.987533
15.222999	770.476551	12.992551
15.089873	769.490816	12.997568
15.171860	771.560238	13.002586
14.897149	772.788379	13.007603
14.931897	767.373907	13.012621
15.037510	774.130499	13.017639
15.108397	770.703634	13.022656
15.132934	770.877949	13.027674
15.082370	778.049358	13.032691
15.329008	758.577735	13.037709
14.964417	771.024866	13.042727
14.368720	772.772274	13.047744
14.996243	759.890369	13.052762
15.121248	768.825516	13.057779
15.214979	775.733674	13.062797
14.936042	769.019642	13.067815
15.011602	770.307494	13.072832
14.975177	762.113229	13.077850
14.882175	770.147914	13.082867
15.020035	766.299746	13.087885
15.044837	771.811126	13.092903
15.108932	768.792451	13.097920
15.235331	766.689392	13.102938
15.128726	774.931439	13.107955
15.396245	770.044927	13.112973
15.256214	769.957925	13.117991
15.072004	768.589725	13.123008
14.854047	760.653461	13.128026
14.942946	775.521036	13.133043
15.190029	777.369825	13.138061
15.405958	784.025088	13.143079
15.498398	792.252688	13.148096
15.515877	780.487473	13.153114
15.096946	774.850893	13.158131
15.193903	769.857591	13.163149
15.527658	780.332503	13.168167
15.046130	786.337943	13.173184
15.533249	783.127178	13.178202
15.369128	799.457068	13.183219
15.340636	793.268454	13.188237
15.556109	798.064055	13.193255
15.362541	807.686194	13.198272
15.755713	798.905449	13.203290
15.460776	790.291795	13.208307
15.587314	772.996618	13.213325
15.400154	763.664384	13.218343
15.679890	769.596910	13.223360
15.445721	769.007807	13.228378
15.454737	768.153252	13.233395
15.501813	773.707398	13.238413
15.475260	784.027813	13.243431
15.475562	791.593540	13.248448
15.734810	794.139098	13.253466
15.694478	791.545562	13.258483
15.557965	792.185103	13.263501
15.480443	788.877292	13.268519
15.444796	795.124634	13.273536
15.804163	795.165558	13.278554
15.693444	800.077374	13.283571
15.915965	791.006796	13.288589
15.883004	792.227584	13.293607
15.563890	793.468985	13.298624
16.111775	788.405735	13.303642
15.918653	791.932449	13.308659
15.776291	775.611667	13.313677
15.742031	763.818420	13.318695
15.540761	774.270902	13.323712
15.548396	779.332790	13.328730
15.472321	788.817359	13.333747
15.779924	787.910999	13.338765
15.873966	789.886306	13.343783
15.727333	800.439596	13.348800
15.943411	787.104171	13.353818
15.704329	787.583540	13.358835
15.629378	794.408226	13.363853
16.018407	786.804489	13.368871
15.895523	791.657690	13.373888
15.808140	794.365363	13.378906
15.776521	792.597112	13.383923
15.763263	793.293406	13.388941
15.708806	786.599279	13.393959
15.810445	800.971881	13.398976
16.218422	809.290542	13.403994
16.379422	815.650993	13.409011
16.019829	798.845318	13.414029
16.359657	798.844203	13.419047
15.869123	801.914681	13.424064
16.050608	797.002252	13.429082
16.254677	796.124846	13.434099
16.001891	791.546911	13.439117
16.294109	785.261497	13.444135
16.044599	800.265835	13.449152
15.887596	797.521547	13.454170
16.316184	808.082738	13.459187
16.299269	821.970687	13.464205
16.563605	817.129174	13.469223
16.058306	805.270593	13.474240
16.191901	794.179806	13.479258
16.545729	807.396542	13.484275
16.176410	802.776092	13.489293
16.429473	787.597238	13.494311
15.896516	795.651245	13.499328
15.675778	797.665291	13.504346
15.369157	813.131436	13.509363
16.144358	818.137102	13.514381
16.548377	817.470668	13.519399
16.192207	819.067401	13.524416
16.524156	822.399310	13.529434
16.222627	822.496127	13.534451
16.180244	820.141102	13.539469
16.538024	823.864777	13.544487
16.709529	825.465863	13.549504
16.836469	819.039702	13.554522
16.982947	821.263404	13.559539
16.583033	822.193399	13.564557
16.684335	817.632018	13.569575
16.649824	819.607751	13.574592
16.888051	814.475695	13.579610
16.709815	814.573355	13.584627
16.818466	816.091546	13.589645
17.158352	799.429876	13.594663
16.637689	801.284935	13.599680
16.669726	795.514621	13.604698
16.876347	782.485081	13.609715
16.376037	780.281081	13.614733
16.829659	781.604752	13.619751
16.531415	794.257833	13.624768
16.811570	796.688912	13.629786
16.919014	783.777756	13.634803
16.345732	796.502757	13.639821
16.891977	793.290860	13.644839
16.633143	808.714052	13.649856
16.887415	807.006328	13.654874
16.778780	816.728970	13.659891
16.730315	818.488127	13.664909
17.109048	814.374877	13.669927
16.895666	811.297814	13.674944
16.838982	812.439859	13.679962
17.243562	815.070012	13.684979
16.722921	811.472202	13.689997
17.016265	781.487067	13.695015
16.555384	806.252267	13.700032
16.906267	812.456479	13.705050
17.158730	809.984134	13.710067
16.999017	811.662109	13.715085
16.715695	812.225966	13.720103
17.062312	810.867499	13.725120
17.126194	808.491731	13.730138
17.185343	811.054678	13.735155
17.037051	815.194021	13.740173
17.029007	805.439603	13.745191
17.047495	810.635523	13.750208
17.000270	808.284058	13.755226
17.166449	802.335632	13.760243
17.206195	817.402322	13.765261
17.315310	812.798705	13.770279
16.894658	815.183634	13.775296
17.210203	812.449281	13.780314
17.050919	810.608077	13.785331
16.583468	811.854751	13.790349
17.138599	809.845648	13.795367
16.814070	818.330090	13.800384
16.514839	812.395343	13.805402
16.977567	818.731817	13.810419
17.197143	836.440658	13.815437
17.632468	834.567919	13.820455
17.411745	839.744407	13.825472
17.823282	837.574441	13.830490
17.693912	810.492173	13.835507
17.141381	806.116615	13.840525
17.366317	804.548388	13.845543
17.262411	808.380788	13.850560
17.375643	806.146841	13.855578
17.704562	801.957990	13.860595
17.169886	807.191176	13.865613
17.455861	802.399231	13.870631
17.503761	806.705287	13.875648
17.385057	804.586119	13.880666
17.542230	803.675929	13.885683
17.576127	808.478767	13.890701
17.554650	801.225264	13.895719
17.329146	808.544546	13.900736
17.129094	823.206089	13.905754
17.696617	824.419570	13.910771
17.563151	827.771462	13.915789
17.691997	827.702926	13.920807
17.513152	833.502366	13.925824
17.157648	832.812098	13.930842
17.842358	828.296230	13.935859
17.800998	837.461710	13.940877
17.932390	827.159413	13.945895
17.586792	832.497513	13.950912
17.624399	831.040613	13.955930
17.887940	821.348296	13.960947
17.617228	833.725998	13.965965
17.956872	824.126978	13.970983
17.763495	826.761662	13.976000
17.725140	834.560177	13.981018
17.828556	823.927886	13.986035
17.655461	831.218029	13.991053
17.944232	828.247962	13.996071
17.835320	831.057233	14.001088
17.832789	833.989041	14.006106
18.131904	816.621935	14.011123
18.043817	828.682400	14.016141
17.623654	826.815497	14.021159
17.532693	831.436271	14.026176
17.374172	828.440273	14.031194
17.814466	833.066382	14.036211
17.954225	855.672860	14.041229
18.132244	856.971704	14.046247
18.209661	846.202372	14.051264
18.356498	848.202801	14.056282
18.746556	837.774599	14.061299
18.380036	826.037109	14.066317
18.366477	824.000917	14.071335
18.526554	815.823690	14.076352
18.646537	816.752240	14.081370
18.573494	816.538796	14.086387
18.309115	817.405012	14.091405
18.465600	805.106552	14.096423
18.644787	804.955669	14.101440
18.072289	796.718662	14.106458
18.300014	790.287241	14.111475
18.282926	805.712917	14.116493
18.386065	805.064417	14.121511
18.340111	808.118758	14.126528
18.195428	804.556329	14.131546
18.583409	810.664639	14.136563
18.143201	806.012227	14.141581
18.480538	806.924863	14.146599
18.414090	808.195683	14.151616
18.332652	808.587142	14.156634
18.301721	812.788542	14.161651
18.351720	827.622847	14.166669
18.201647	819.475716	14.171687
18.248482	818.383018	14.176704
18.410244	817.215781	14.181722
18.612316	805.023546	14.186739
18.397509	819.086773	14.191757
18.528323	817.630187	14.196775
18.504862	814.977164	14.201792
18.257732	822.544115	14.206810
18.685788	820.531644	14.211827
18.635248	822.246659	14.216845
18.439605	817.473830	14.221863
18.496634	820.381994	14.226880
18.114634	819.666194	14.231898
18.327902	817.926285	14.236915
18.232312	841.353955	14.241933
18.489697	845.772178	14.246951
18.729268	852.316475	14.251968
18.727094	847.694663	14.256986
18.785370	843.294722	14.262003
18.919948	850.481176	14.267021
18.788762	856.433748	14.272039
18.911030	850.712250	14.277056
18.966443	856.068205	14.282074
18.999241	846.276685	14.287091
19.083787	851.484908	14.292109
18.994280	850.395100	14.297127
19.021197	839.951440	14.302144
19.090282	852.964197	14.307162
19.207548	848.764318	14.312179
18.844005	852.279109	14.317197
18.844726	843.270423	14.322215
18.974401	852.467431	14.327232
19.080790	839.562702	14.332250
19.362033	841.626304	14.337267
18.853127	845.742300	14.342285
18.898970	847.427579	14.347303
19.124830	833.622014	14.352320
19.074481	837.597514	14.357338
19.046758	837.576163	14.362355
19.083748	842.472982	14.367373
18.788644	845.262301	14.372391
19.169572	847.712921	14.377408
18.989386	858.092287	14.382426
19.291293	844.467418	14.387443
19.057508	841.696074	14.392461
18.765407	841.528744	14.397479
18.986476	846.778530	14.402496
19.045620	855.407326	14.407514
19.251296	862.621381	14.412531
19.167445	870.176672	14.417549
19.397765	875.436353	14.422567
19.565887	876.749830	14.427584
19.605840	871.419101	14.432602
19.661357	868.011294	14.437619
19.412925	849.495112	14.442637
19.126449	839.530096	14.447655
19.551151	850.572645	14.452672
19.488496	866.817698	14.457690
19.583212	870.324326	14.462707
19.714180	872.142750	14.467725
19.327611	864.319780	14.472743
19.462004	858.078580	14.477760
19.632145	870.360086	14.482778
19.695290	862.406355	14.487795
19.504832	875.597926	14.492813
19.343156	871.959560	14.497831
19.543950	864.892440	14.502848
19.554229	875.514282	14.507866
19.676688	870.141547	14.512883
19.879305	869.557671	14.517901
19.596733	874.715672	14.522919
19.765734	863.220961	14.527936
19.477841	874.528364	14.532954
19.741739	861.429827	14.537971
19.536502	876.611151	14.542989
19.417614	874.450274	14.548007
19.865463	863.174337	14.553024
19.497641	875.402412	14.558042
19.562405	875.197644	14.563059
19.577504	870.545014	14.568077
19.745030	873.398673	14.573095
19.785732	879.048003	14.578112
19.564446	903.244969	14.583130
20.252951	897.137188	14.588147
20.204386	893.308835	14.593165
20.006983	895.981203	14.598183
20.094385	888.256502	14.603200
20.549045	893.761706	14.608218
20.380514	870.221480	14.613235
20.519413	857.793613	14.618253
20.210810	859.672223	14.623271
20.492624	854.816387	14.628288
20.244817	856.391637	14.633306
20.211419	855.086643	14.638323
20.569248	859.703581	14.643341
20.106013	857.735151	14.648359
20.404267	846.142282	14.653376
20.037736	861.512495	14.658394
20.122359	860.228507	14.663411
20.349300	851.165036	14.668429
20.386195	851.743191	14.673447
20.359558	858.364639	14.678464
20.150671	862.497887	14.683482
20.404797	850.818231	14.688499
20.148056	845.846072	14.693517
20.253429	856.478926	14.698535
20.264901	860.510727	14.703552
20.222896	859.494152	14.708570
20.063056	854.666567	14.713587
20.149631	859.032372	14.718605
19.882806	858.182938	14.723623
20.224855	862.480852	14.728640
19.951003	881.841451	14.733658
20.051059	890.329640	14.738675
20.356153	882.079156	14.743693
20.390216	893.324208	14.748711
20.459734	884.005301	14.753728
20.708720	895.097843	14.758746
20.878861	895.903531	14.763763
21.388021	885.464237	14.768781
20.582364	890.012827	14.773799
20.940569	888.643381	14.778816
20.820475	892.452106	14.783834
20.781510	896.712337	14.788851
21.070111	881.255866	14.793869
21.091659	890.742048	14.798887
21.129137	885.974690	14.803904
21.045935	867.041382	14.808922
20.525726	853.844745	14.813939
20.887156	847.268726	14.818957
20.684552	849.851795	14.823975
21.090180	851.864095	14.828992
21.066624	854.772617	14.834010
20.774837	853.169086	14.839027
20.839952	854.345688	14.844045
20.695207	863.307447	14.849063
21.143808	865.561440	14.854080
20.721643	864.166889	14.859098
20.913289	881.164299	14.864115
21.104735	883.482528	14.869133
20.925107	886.957818	14.874151
20.903774	880.759717	14.879168
20.834878	894.346116	14.884186
21.048676	892.444308	14.889203
21.150472	884.270003	14.894221
21.036883	896.075700	14.899239
20.963485	883.008981	14.904256
21.036284	888.483716	14.909274
20.856579	897.176494	14.914291
21.417515	882.247736	14.919309
21.043850	878.775959	14.924327
21.341947	885.593637	14.929344
21.360189	886.700447	14.934362
21.210465	900.016784	14.939379
21.234579	888.718871	14.944397
21.295912	897.221350	14.949415
21.382490	885.325722	14.954432
21.070803	894.105703	14.959450
21.105313	890.328947	14.964467
21.129782	892.520108	14.969485
21.285154	917.298793	14.974503
21.856708	907.643212	14.979520
21.715339	919.458251	14.984538
21.565597	914.312061	14.989555
21.271791	901.100728	14.994573
21.340254	915.695457	14.999591
21.736734	912.124495	15.004608
21.685701	909.164617	15.009626
21.631167	917.248912	15.014643
21.613697	909.342756	15.019661
21.759744	915.094335	15.024679
21.570293	899.340642	15.029696
21.704766	898.083041	15.034714
21.312248	912.336006	15.039731
21.828121	907.029212	15.044749
21.702497	907.739393	15.049767
21.645444	902.107014	15.054784
21.853578	902.413521	15.059802
21.769558	906.714678	15.064819
21.848648	903.295480	15.069837
21.618416	911.713574	15.074855
21.747801	899.675027	15.079872
21.945501	905.270025	15.084890
21.806275	915.431239	15.089907
21.999113	900.977174	15.094925
22.028865	909.192383	15.099943
22.160815	909.524496	15.104960
21.787157	912.416594	15.109978
21.483250	913.871617	15.114995
21.869520	906.005299	15.120013
21.760463	916.999669	15.125031
22.038686	918.864184	15.130048
22.357688	929.715247	15.135066
21.888372	929.302075	15.140083
22.109217	929.159253	15.145101
22.099177	943.151286	15.150119
22.570291	939.673467	15.155136
22.651335	924.368245	15.160154
22.277491	915.743965	15.165171
22.517978	912.619285	15.170189
22.104312	900.572630	15.175207
21.920476	902.771121	15.180224
22.031180	899.271890	15.185242
22.087721	921.092280	15.190259
22.268340	916.863390	15.195277
22.447244	939.461147	15.200295
22.405965	935.750470	15.205312
22.464021	938.059299	15.210330
22.132637	939.064170	15.215347
22.357181	928.533793	15.220365
21.905818	936.305869	15.225383
22.177525	933.060667	15.230400
22.658949	935.639536	15.235418
22.296030	932.778145	15.240435
22.618022	937.187665	15.245453
22.605392	934.699356	15.250471
22.402363	936.647104	15.255488
22.484835	931.930546	15.260506
22.610046	942.793235	15.265523
22.329153	932.330405	15.270541
22.648845	942.456198	15.275559
22.751003	952.861313	15.280576
22.794865	953.086364	15.285594
22.664423	946.112243	15.290611
23.061367	939.292520	15.295629
22.858304	928.221163	15.300647
23.033816	927.586657	15.305664
23.049840	924.402296	15.310682
22.963607	929.825824	15.315699
22.855676	922.218092	15.320717
22.757452	920.942329	15.325735
23.038346	916.849584	15.330752
23.243777	912.008347	15.335770
23.004789	914.562413	15.340787
23.208075	911.378149	15.345805
23.081386	919.757450	15.350823
23.076856	927.951181	15.355840
23.312447	911.205090	15.360858
23.148902	918.999969	15.365875
23.117630	912.559417	15.370893
23.364235	924.077158	15.375911
23.252847	919.156101	15.380928
23.407174	920.335258	15.385946
23.344667	921.688895	15.390963
23.603814	920.580719	15.395981
23.424953	916.195221	15.400999
23.210897	923.691394	15.406016
23.519709	916.829583	15.411034
23.506230	919.136083	15.416051
23.406688	904.873335	15.421069
23.519330	891.424638	15.426087
23.316253	892.168508	15.431104
23.202866	878.480885	15.436122
23.006094	902.190349	15.441139
23.547425	905.181322	15.446157
23.359774	918.576787	15.451175
23.456719	909.785189	15.456192
23.317220	903.781046	15.461210
23.101999	913.680445	15.466227
23.238897	910.024519	15.471245
23.496262	910.340590	15.476263
23.120326	908.708074	15.481280
23.400721	905.690563	15.486298
23.026957	914.476897	15.491315
23.374235	920.743952	15.496333
23.338271	936.077613	15.501351
23.412413	937.924351	15.506368
23.456015	935.674751	15.511386
23.484220	943.363879	15.516403
23.503382	937.657846	15.521421
23.484626	942.857222	15.526439
23.797128	955.591187	15.531456
24.254252	951.957815	15.536474
23.958904	944.264181	15.541491
24.113519	932.894235	15.546509
23.968577	933.222199	15.551527
23.686270	931.911959	15.556544
23.822557	936.514819	15.561562
23.668258	932.850414	15.566579
23.928450	934.304156	15.571597
24.108288	940.505642	15.576615
24.111155	936.217207	15.581632
23.997111	937.231363	15.586650
23.677195	940.940122	15.591667
23.984422	950.827049	15.596685
24.468203	959.407638	15.601703
24.419833	963.251746	15.606720
24.410124	954.743913	15.611738
24.127023	941.881939	15.616755
24.246115	928.863226	15.621773
23.872586	928.683001	15.626791
24.262137	941.677020	15.631808
24.471671	943.692276	15.636826
24.125229	958.579753	15.641843
24.695955	958.164045	15.646861
24.719885	952.883577	15.651879
24.350350	938.680070	15.656896
24.554831	929.224227	15.661914
24.308906	926.983200	15.666931
24.524035	921.159689	15.671949
24.135071	915.354322	15.676967
24.386200	937.553521	15.681984
24.892591	947.264955	15.687002
24.476967	943.914672	15.692019
24.473093	945.056644	15.697037
24.454258	944.000007	15.702055
24.697188	955.987651	15.707072
24.965639	946.204683	15.712090
24.441714	939.896479	15.717107
24.858322	950.790054	15.722125
24.875725	944.241433	15.727143
24.455163	935.620940	15.732160
24.804907	939.431010	15.737178
24.854994	954.455178	15.742195
24.672639	954.722411	15.747213
24.855723	947.400717	15.752231
24.807901	947.864169	15.757248
24.901229	952.521783	15.762266
24.708430	955.862268	15.767283
24.627733	953.852529	15.772301
24.913690	950.062861	15.777319
24.778241	949.716842	15.782336
24.875556	945.146241	15.787354
24.690141	960.571205	15.792371
24.532019	950.584470	15.797389
24.861959	946.781615	15.802407
24.828772	954.718700	15.807424
25.110645	965.725536	15.812442
25.078531	971.398373	15.817459
24.796266	983.411587	15.822477
25.232040	983.119008	15.827495
24.989505	979.247558	15.832512
25.406128	969.398704	15.837530
25.199429	974.989038	15.842547
25.465106	978.655564	15.847565
25.431820	975.265587	15.852583
25.245776	974.427966	15.857600
25.443714	972.973637	15.862618
25.098328	971.593132	15.867635
25.190246	971.374812	15.872653
25.677570	966.621915	15.877671
25.092632	976.878624	15.882688
25.340488	966.740407	15.887706
25.109227	974.796910	15.892723
25.285824	963.276851	15.897741
25.362560	967.891157	15.902759
25.078507	973.683661	15.907776
25.399456	981.594009	15.912794
25.950761	994.351848	15.917811
25.739103	989.602483	15.922829
25.895294	972.339968	15.927847
25.715045	969.734925	15.932864
26.021884	974.158382	15.937882
25.793341	961.517269	15.942899
25.774063	961.451607	15.947917
25.913213	961.719934	15.952935
25.676682	969.470233	15.957952
25.730365	966.930782	15.962970
25.605223	959.893180	15.967987
25.612679	968.735315	15.973005
26.207009	975.283125	15.978023
25.988972	981.473346	15.983040
25.691779	969.556163	15.988058
26.046470	971.613920	15.993075
26.136730	988.253842	15.998093
26.171934	976.413499	16.003111
26.000998	970.217693	16.008128
26.424558	962.932942	16.013146
26.086448	965.188481	16.018163
26.077861	961.038545	16.023181
26.218012	955.964019	16.028199
25.975440	965.854595	16.033216
25.882110	979.477791	16.038234
25.925718	986.465995	16.043251
26.288220	992.947873	16.048269
26.291055	987.112641	16.053287
26.234074	1003.046280	16.058304
26.103447	990.928279	16.063322
26.184330	1000.417695	16.068339
25.911022	995.348628	16.073357
26.402708	983.990153	16.078375
26.477720	993.128976	16.083392
26.273453	990.251146	16.088410
26.274503	992.539504	16.093427
26.021664	986.424573	16.098445
26.808667	994.664040	16.103463
26.686080	1007.983063	16.108480
26.639721	998.895471	16.113498
27.023014	990.775282	16.118515
26.894075	992.995797	16.123533
26.443879	984.635685	16.128551
26.412288	991.748542	16.133568
26.577963	980.520425	16.138586
26.817069	981.091479	16.143603
26.807742	1004.523222	16.148621
26.986739	993.832239	16.153639
26.891097	989.916779	16.158656
26.901513	981.202457	16.163674
26.936548	982.370271	16.168691
26.823625	988.379711	16.173709
26.883980	989.120908	16.178727
26.789414	1002.384501	16.183744
26.859745	1004.588557	16.188762
27.411134	1021.052164	16.193779
27.127027	1008.432417	16.198797
27.253078	991.249278	16.203815
26.754696	996.598559	16.208832
26.777989	987.501408	16.213850
27.390743	1004.396945	16.218867
27.138102	1011.050763	16.223885
27.329252	998.206667	16.228903
26.798846	991.503467	16.233920
26.969583	998.749355	16.238938
26.945306	1008.806561	16.243955
27.093805	1009.256797	16.248973
27.410670	1000.725572	16.253991
27.428606	1008.354231	16.259008
27.670371	1007.767805	16.264026
27.780658	1001.717145	16.269043
27.772912	1006.493870	16.274061
27.303604	994.251244	16.279079
27.389368	974.984326	16.284096
27.373971	987.846231	16.289114
27.750586	1000.686936	16.294131
27.594157	994.504859	16.299149
27.604318	976.932674	16.304167
27.577011	974.046411	16.309184
27.396039	973.490615	16.314202
27.583651	975.889804	16.319219
27.484256	992.644202	16.324237
27.864940	995.174805	16.329255
27.748071	998.873578	16.334272
27.731894	1007.177937	16.339290
27.610047	1005.985996	16.344307
27.289604	1008.569312	16.349325
28.019800	1005.971771	16.354343
27.939999	999.412845	16.359360
27.643501	1000.146599	16.364378
27.817089	995.103530	16.369395
27.690408	1000.914867	16.374413
27.629352	997.517279	16.379431
27.739164	994.418946	16.384448
27.806018	997.109777	16.389466
27.728545	997.863955	16.394483
27.668209	1025.893758	16.399501
28.034216	1027.389828	16.404519
28.209631	1023.403888	16.409536
28.056569	1031.887613	16.414554
28.344895	1024.516174	16.419571
27.903416	1027.810059	16.424589
28.341900	1030.119688	16.429607
28.077869	1028.841844	16.434624
28.067269	1029.334566	16.439642
28.193621	1030.824652	16.444659
28.027327	1029.388504	16.449677
28.317854	1034.622916	16.454695
27.843338	1020.704817	16.459712
28.302766	1030.493762	16.464730
28.701522	1035.932687	16.469747
28.225173	1036.584809	16.474765
28.415556	1041.163784	16.479783
28.380943	1049.665305	16.484800
28.284187	1052.218676	16.489818
28.514694	1066.780024	16.494835
28.374584	1057.231560	16.499853
28.776888	1047.411405	16.504871
29.098209	1045.841761	16.509888
28.573019	1048.442845	16.514906
28.996287	1048.943252	16.519923
28.881910	1049.183089	16.524941
28.972861	1044.375333	16.529959
29.151072	1046.356027	16.534976
29.140009	1042.450564	16.539994
28.756597	1018.333510	16.545011
28.889623	1014.494349	16.550029
29.107467	1013.810313	16.555047
29.010700	1009.046642	16.560064
28.555290	1007.622149	16.565082
29.028153	1016.504960	16.570099
28.934922	1031.889535	16.575117
29.238230	1027.325352	16.580135
29.161761	1027.514425	16.585152
28.644830	1030.991270	16.590170
29.216557	1033.545756	16.595187
28.975851	1038.689793	16.600205
29.358579	1042.592062	16.605223
29.489328	1050.173716	16.610240
29.394949	1041.791268	16.615258
29.350442	1036.592574	16.620275
29.189564	1022.165470	16.625293
28.982798	1026.575171	16.630311
29.267194	1040.465391	16.635328
29.536369	1046.811964	16.640346
29.788408	1036.402153	16.645363
29.350439	1037.877810	16.650381
29.508940	1040.711342	16.655399
29.544287	1042.681834	16.660416
29.682716	1043.408926	16.665434
29.817558	1028.530504	16.670451
29.431756	1016.959833	16.675469
29.132925	1018.353790	16.680487
29.504395	1028.475397	16.685504
29.317902	1045.525366	16.690522
29.293299	1030.891051	16.695539
29.666513	1042.514683	16.700557
29.667985	1039.382707	16.705575
29.820120	1034.327824	16.710592
29.363815	1039.674089	16.715610
29.894403	1030.599604	16.720627
29.715197	1038.841214	16.725645
29.560229	1042.558510	16.730663
29.927369	1051.907649	16.735680
29.907765	1070.506726	16.740698
30.244031	1068.614145	16.745715
29.580963	1065.874865	16.750733
29.708111	1065.842829	16.755751
30.529733	1070.751922	16.760768
30.171306	1072.217168	16.765786
30.540542	1069.786862	16.770803
30.044480	1069.693457	16.775821
30.018971	1066.951362	16.780839
30.500793	1063.861493	16.785856
30.224205	1072.040508	16.790874
30.658182	1063.653237	16.795891
30.303157	1044.980066	16.800909
30.163729	1034.714994	16.805927
30.081676	1044.319996	16.810944
30.096208	1055.192823	16.815962
30.584414	1056.776926	16.820979
30.707952	1066.358923	16.825997
30.573694	1068.345298	16.831015
30.704036	1059.010704	16.836032
30.385978	1063.072320	16.841050
30.577356	1059.452218	16.846067
30.394131	1070.913293	16.851085
30.568833	1061.316243	16.856103
31.098494	1064.491457	16.861120
30.528178	1066.273273	16.866138
30.853245	1053.294756	16.871155
30.864566	1060.106849	16.876173
30.653399	1071.501688	16.881191
31.058833	1055.989872	16.886208
30.705644	1068.965255	16.891226
30.789199	1050.498581	16.896243
30.727774	1054.671633	16.901261
30.931889	1052.795817	16.906279
31.132240	1050.246633	16.911296
30.938170	1067.617161	16.916314
31.028520	1054.156660	16.921331
30.780669	1057.688953	16.926349
30.969193	1054.568126	16.931367
31.138046	1049.371105	16.936384
30.907492	1059.533757	16.941402
30.961816	1054.112399	16.946419
31.092820	1052.382149	16.951437
30.812467	1060.207463	16.956455
31.057615	1049.083456	16.961472
30.921827	1051.473611	16.966490
30.996102	1041.966427	16.971507
31.071419	1059.574219	16.976525
31.103620	1069.818563	16.981543
31.419662	1068.602141	16.986560
31.378763	1077.702336	16.991578
31.127430	1073.755942	16.996595
31.388449	1072.698232	17.001613
31.296779	1074.557482	17.006631
31.503840	1066.943189	17.011648
31.676232	1076.470255	17.016666
31.703599	1072.360002	17.021683
31.720699	1077.748755	17.026701
31.653911	1076.976417	17.031719
31.532827	1067.608254	17.036736
31.631815	1077.087634	17.041754
31.927636	1069.848394	17.046771
31.759826	1076.441344	17.051789
31.797766	1072.889951	17.056807
31.812275	1064.988656	17.061824
31.640226	1077.686031	17.066842
31.855893	1079.669189	17.071859
32.123584	1063.721527	17.076877
31.785421	1082.619420	17.081895
31.877119	1075.088003	17.086912
31.811807	1080.368753	17.091930
32.225210	1083.074656	17.096947
32.314190	1083.806395	17.101965
31.932396	1077.949779	17.106983
32.327192	1072.505110	17.112000
32.047432	1070.500364	17.117018
31.932932	1091.009600	17.122035
32.331852	1096.212701	17.127053
31.972850	1104.600648	17.132071
32.119229	1104.762272	17.137088
31.688875	1093.097349	17.142106
32.480322	1101.339289	17.147123
32.361624	1099.834232	17.152141
32.679747	1099.931986	17.157159
32.570765	1090.398819	17.162176
32.548953	1101.822560	17.167194
32.365684	1090.072240	17.172211
32.702136	1091.411012	17.177229
32.524394	1097.111946	17.182247
32.765481	1088.955412	17.187264
32.782580	1095.620900	17.192282
32.688770	1097.532867	17.197299
32.481839	1099.316719	17.202317
32.275554	1101.398880	17.207335
32.633739	1089.256554	17.212352
32.810909	1095.370752	17.217370
32.701160	1096.246810	17.222387
32.536472	1096.194989	17.227405
32.692519	1115.503987	17.232423
32.818487	1124.595870	17.237440
32.827158	1125.538933	17.242458
33.192828	1115.767319	17.247475
33.223961	1111.691078	17.252493
32.864309	1126.799399	17.257511
33.252511	1108.392445	17.262528
33.358720	1117.135638	17.267546
33.133299	1113.776657	17.272563
33.585561	1110.533805	17.277581
33.713464	1107.766695	17.282599
33.382982	1082.504199	17.287616
33.418103	1080.672896	17.292634
32.993982	1084.108795	17.297651
33.320292	1087.744837	17.302669
33.074494	1085.610454	17.307687
33.483903	1089.591386	17.312704
33.696382	1105.014781	17.317722
33.237861	1102.864440	17.322739
33.908063	1100.981126	17.327757
33.494373	1093.071981	17.332775
33.498345	1081.689075	17.337792
33.609298	1083.562018	17.342810
33.836188	1095.643369	17.347827
34.276163	1084.557547	17.352845
33.407742	1092.292855	17.357863
33.728657	1073.179785	17.362880
33.464503	1072.714133	17.367898
33.428266	1088.138539	17.372915
33.836522	1089.723286	17.377933
33.534821	1100.555597	17.382951
33.980066	1100.294125	17.387968
33.648910	1106.339351	17.392986
33.804208	1103.829114	17.398003
33.849273	1098.728949	17.403021
33.909649	1105.501051	17.408039
34.127280	1102.280122	17.413056
33.803927	1098.414149	17.418074
33.530897	1098.644432	17.423091
33.807677	1109.100658	17.428109
33.839371	1127.128335	17.433127
33.984975	1136.118552	17.438144
34.263314	1142.939223	17.443162
33.932827	1130.752238	17.448179
34.224355	1124.921907	17.453197
34.540608	1130.090678	17.458215
34.507645	1128.121435	17.463232
34.602751	1133.282338	17.468250
34.826456	1122.773227	17.473267
34.828465	1122.015479	17.478285
34.917765	1132.785826	17.483303
34.615742	1132.944533	17.488320
34.495194	1125.312413	17.493338
34.642812	1121.687338	17.498355
34.887995	1119.444884	17.503373
34.618205	1131.022695	17.508391
34.787303	1118.445922	17.513408
34.425150	1125.543499	17.518426
34.739471	1131.407450	17.523443
34.793725	1120.674831	17.528461
34.839755	1121.126684	17.533479
34.914292	1118.557772	17.538496
35.286173	1118.829297	17.543514
34.806032	1125.517684	17.548531
34.844618	1119.712701	17.553549
34.737215	1126.596843	17.558567
34.997041	1125.122805	17.563584
35.189592	1118.457710	17.568602
34.742564	1127.580300	17.573619
35.013448	1123.700570	17.578637
35.060996	1125.996208	17.583655
35.144306	1127.032815	17.588672
35.260159	1143.800160	17.593690
35.397202	1140.896888	17.598707
35.493556	1136.197261	17.603725
35.288660	1124.691039	17.608743
35.208459	1126.384621	17.613760
35.723399	1131.163812	17.618778
35.216770	1132.391799	17.623795
35.431863	1140.352827	17.628813
35.688209	1144.154399	17.633831
35.602042	1146.278486	17.638848
35.564412	1132.889107	17.643866
35.434280	1138.182185	17.648883
35.553269	1135.214977	17.653901
35.840221	1137.277675	17.658919
35.806263	1136.816030	17.663936
35.901525	1143.654811	17.668954
35.971540	1147.938010	17.673971
35.865484	1140.025538	17.678989
35.683452	1141.700158	17.684007
35.863612	1130.217573	17.689024
35.977064	1134.683728	17.694042
35.889781	1133.397868	17.699059
35.897708	1135.787860	17.704077
35.876305	1137.026840	17.709095
35.997656	1130.161725	17.714112
35.909270	1132.142087	17.719130
35.494411	1137.475223	17.724147
35.973799	1140.328080	17.729165
36.277078	1155.593976	17.734183
36.152317	1158.168143	17.739200
36.464866	1164.809542	17.744218
36.255970	1173.071887	17.749235
36.300981	1164.228116	17.754253
36.221112	1170.839616	17.759271
36.339411	1173.062918	17.764288
36.885996	1162.100329	17.769306
36.776324	1159.028856	17.774323
36.873652	1160.187944	17.779341
36.550962	1148.932303	17.784359
36.478394	1158.189753	17.789376
36.801918	1147.566069	17.794394
36.609301	1152.524233	17.799411
36.702891	1153.606775	17.804429
36.831124	1148.750296	17.809447
36.869609	1151.069484	17.814464
36.743756	1154.022953	17.819482
36.311204	1155.554021	17.824499
36.672466	1147.688967	17.829517
36.800120	1159.650190	17.834535
36.735333	1164.451762	17.839552
37.124849	1151.718391	17.844570
36.509457	1155.453290	17.849587
36.793147	1157.679518	17.854605
36.853912	1163.543734	17.859623
36.858706	1171.638023	17.864640
37.077385	1181.500392	17.869658
36.849121	1186.268806	17.874675
36.898637	1183.670562	17.879693
36.928966	1182.088854	17.884711
37.061223	1187.076305	17.889728
37.507861	1181.849779	17.894746
37.431929	1183.769032	17.899763
37.198795	1179.334966	17.904781
37.538838	1193.421223	17.909799
37.517406	1201.717108	17.914816
37.670168	1204.649650	17.919834
37.664713	1203.723847	17.924851
37.453004	1192.334054	17.929869
37.771636	1191.993548	17.934887
37.510446	1204.244775	17.939904
38.056798	1199.060393	17.944922
37.724848	1190.354613	17.949939
37.759937	1186.980826	17.954957
37.535805	1184.210576	17.959975
37.537977	1201.059403	17.964992
38.072600	1208.228602	17.970010
37.942866	1215.465684	17.975027
37.948092	1199.312530	17.980045
37.862392	1195.308759	17.985063
38.093254	1207.119469	17.990080
38.366872	1205.481333	17.995098
38.184726	1203.816697	18.000115
37.950356	1197.746653	18.005133
38.513614	1202.340312	18.010151
38.148669	1213.337106	18.015168
38.526043	1197.964043	18.020186
38.234942	1201.331093	18.025203
38.272312	1212.993929	18.030221
38.315558	1202.998883	18.035239
38.236097	1209.308765	18.040256
38.578749	1196.170135	18.045274
38.699178	1213.022622	18.050291
38.559680	1206.041614	18.055309
38.568540	1203.191838	18.060327
38.269142	1204.465042	18.065344
38.541715	1194.845011	18.070362
38.574393	1210.109312	18.075379
38.671036	1198.597593	18.080397
38.734862	1192.173854	18.085415
38.443284	1204.235236	18.090432
38.558047	1197.789675	18.095450
38.831899	1213.970320	18.100467
38.643551	1223.614292	18.105485
38.436184	1219.990888	18.110503
38.720210	1230.321591	18.115520
38.875318	1220.136757	18.120538
38.883389	1228.047465	18.125555
38.777426	1221.266798	18.130573
38.855704	1227.060817	18.135591
39.076954	1254.713710	18.140608
39.324891	1252.770773	18.145626
39.315737	1251.710150	18.150643
39.245478	1251.728517	18.155661
39.593686	1251.855150	18.160679
39.602026	1242.461514	18.165696
40.153286	1236.866474	18.170714
39.484999	1229.223818	18.175731
39.486026	1209.548602	18.180749
40.113980	1204.441649	18.185767
40.044068	1212.223927	18.190784
39.949375	1212.278229	18.195802
39.893482	1205.515261	18.200819
39.833406	1203.814665	18.205837
39.607567	1202.989524	18.210855
39.163851	1207.713699	18.215872
39.658218	1208.291708	18.220890
39.395353	1212.872950	18.225907
39.482818	1210.487311	18.230925
39.621359	1201.492209	18.235943
39.876647	1222.209280	18.240960
40.006880	1227.397074	18.245978
39.932538	1235.833231	18.250995
40.002758	1239.489272	18.256013
40.108772	1240.244181	18.261031
40.070341	1242.093848	18.266048
39.864141	1242.120157	18.271066
40.381753	1238.726699	18.276083
40.274630	1234.977640	18.281101
40.402753	1234.435613	18.286119
39.977015	1241.887856	18.291136
40.280378	1240.141251	18.296154
40.440244	1232.632721	18.301171
40.050652	1227.404095	18.306189
40.307939	1229.470930	18.311207
40.386506	1236.421963	18.316224
40.470458	1228.518535	18.321242
40.426401	1225.819639	18.326259
40.071801	1227.831101	18.331277
40.452318	1246.600747	18.336295
40.445756	1262.653861	18.341312
40.959440	1247.679824	18.346330
40.681141	1251.730575	18.351347
40.990091	1265.433080	18.356365
41.408706	1252.942833	18.361383
40.924650	1257.246940	18.366400
40.891117	1254.545903	18.371418
41.076359	1248.762652	18.376435
41.251150	1252.756490	18.381453
41.866876	1245.143341	18.386471
41.171612	1241.061359	18.391488
41.170464	1220.218014	18.396506
41.366718	1219.749350	18.401523
40.943671	1235.556052	18.406541
41.444186	1228.101747	18.411559
41.192461	1244.495430	18.416576
41.307727	1255.782811	18.421594
41.157611	1241.291516	18.426611
40.970928	1257.018946	18.431629
41.409336	1241.640459	18.436647
41.146489	1249.698004	18.441664
41.160171	1244.644324	18.446682
41.307612	1256.600772	18.451699
41.228328	1258.813889	18.456717
41.308468	1269.759467	18.461735
41.564478	1283.327843	18.466752
41.459483	1282.730715	18.471770
41.760301	1275.916133	18.476787
41.609852	1275.000948	18.481805
41.698380	1278.657116	18.486823
41.573468	1272.847653	18.491840
42.179360	1290.338724	18.496858
42.213304	1291.888623	18.501875
41.729760	1279.472145	18.506893
42.370849	1287.954433	18.511911
42.212618	1306.161795	18.516928
42.437136	1297.944118	18.521946
41.974807	1292.917273	18.526963
41.812004	1296.692617	18.531981
42.265496	1300.230488	18.536999
42.341611	1311.534628	18.542016
42.295465	1305.305819	18.547034
42.486926	1306.045009	18.552051
42.034888	1304.237258	18.557069
42.648737	1297.558627	18.562087
42.684928	1312.922446	18.567104
42.687766	1299.748264	18.572122
42.703709	1301.472008	18.577139
42.614025	1306.689943	18.582157
42.789235	1296.341104	18.587175
42.412262	1310.562333	18.592192
42.298835	1298.828241	18.597210
42.899358	1295.445058	18.602227
42.581990	1300.020783	18.607245
43.103991	1290.945995	18.612263
42.914913	1296.907535	18.617280
42.846665	1295.789765	18.622298
42.813429	1303.477042	18.627315
42.860188	1319.408003	18.632333
43.146430	1317.783514	18.637351
42.363928	1325.990525	18.642368
42.764958	1325.802119	18.647386
43.401659	1321.171231	18.652403
43.300374	1330.253621	18.657421
43.863816	1319.292462	18.662439
43.767128	1323.642288	18.667456
43.734775	1316.281291	18.672474
44.188729	1322.635178	18.677491
44.020816	1317.568237	18.682509
43.890633	1301.249212	18.687527
44.050684	1281.668043	18.692544
43.852049	1281.384838	18.697562
43.934406	1281.320062	18.702579
43.866309	1281.247916	18.707597
43.893235	1276.534546	18.712615
44.014160	1276.699205	18.717632
44.056244	1278.989078	18.722650
43.744487	1279.205302	18.727667
44.015701	1272.295232	18.732685
44.005037	1265.868836	18.737703
43.787302	1270.611123	18.742720
43.845794	1277.372589	18.747738
43.669165	1283.282851	18.752755
43.697141	1283.035351	18.757773
44.015301	1273.863225	18.762791
44.068449	1299.881078	18.767808
43.886711	1302.690682	18.772826
44.339475	1299.687074	18.777843
43.847586	1313.615135	18.782861
44.089132	1307.020192	18.787879
44.049126	1306.472144	18.792896
43.982531	1312.733481	18.797914
44.376403	1311.919502	18.802931
43.978478	1328.547712	18.807949
44.325196	1329.991104	18.812967
44.717764	1335.935483	18.817984
44.956658	1344.837147	18.823002
44.863721	1329.156403	18.828019
44.859286	1337.523167	18.833037
44.815040	1339.574592	18.838055
44.867614	1336.811252	18.843072
44.842905	1340.187371	18.848090
44.911742	1333.187951	18.853107
44.840024	1338.284027	18.858125
44.936553	1327.587964	18.863143
45.110072	1323.631002	18.868160
44.768468	1328.255629	18.873178
45.205954	1338.521232	18.878195
45.170569	1357.115786	18.883213
45.324106	1354.740444	18.888231
45.291459	1361.217043	18.893248
44.993285	1359.978287	18.898266
45.295623	1367.132087	18.903283
45.211654	1356.672187	18.908301
45.608634	1353.065612	18.913319
45.641294	1353.692517	18.918336
45.378662	1350.892392	18.923354
45.457201	1354.702198	18.928371
45.296091	1360.050873	18.933389
45.519278	1353.536902	18.938407
45.591817	1345.711681	18.943424
45.748105	1366.269356	18.948442
46.004318	1371.571377	18.953459
46.064561	1374.087388	18.958477
45.990226	1368.161248	18.963495
45.836212	1358.613717	18.968512
45.689134	1369.803284	18.973530
46.176312	1377.157582	18.978547
45.877674	1382.041642	18.983565
46.129958	1371.614244	18.988583
46.255880	1375.371329	18.993600
46.449533	1379.490816	18.998618
46.676881	1363.166068	19.003635
46.552710	1365.473640	19.008653
46.576223	1364.336341	19.013671
46.565283	1357.052486	19.018688
46.588387	1351.116125	19.023706
46.551129	1336.200550	19.028723
46.248712	1347.765421	19.033741
46.510537	1351.898809	19.038759
46.962752	1362.173407	19.043776
46.819713	1363.734508	19.048794
46.889940	1354.630946	19.053811
46.736915	1366.220306	19.058829
46.847535	1363.509949	19.063847
47.269480	1363.533037	19.068864
46.885470	1361.938814	19.073882
47.238130	1348.966900	19.078899
46.742611	1357.223258	19.083917
46.920141	1349.742455	19.088935
47.396537	1351.120284	19.093952
47.200465	1363.526599	19.098970
47.419348	1358.434969	19.103987
47.075677	1362.358779	19.109005
47.005521	1363.810570	19.114023
47.326090	1358.011563	19.119040
47.287895	1363.328471	19.124058
47.279733	1352.791849	19.129075
47.394300	1367.377797	19.134093
47.186707	1362.166626	19.139111
47.462918	1360.446551	19.144128
47.299355	1364.089757	19.149146
47.722350	1358.059621	19.154163
47.497077	1373.260103	19.159181
47.197259	1382.159650	19.164199
47.459175	1392.533887	19.169216
47.052537	1391.744183	19.174234
47.602761	1385.842575	19.179251
47.946010	1396.379329	19.184269
47.937402	1412.026250	19.189287
48.222563	1403.124469	19.194304
48.301768	1405.927105	19.199322
48.305049	1401.647921	19.204339
48.152028	1399.837891	19.209357
48.227972	1398.972613	19.214375
48.446962	1390.851470	19.219392
48.286917	1403.191616	19.224410
48.522974	1397.588476	19.229427
48.133854	1407.875640	19.234445
48.560397	1406.038937	19.239463
48.854173	1407.043471	19.244480
48.580736	1407.853343	19.249498
48.666154	1413.037990	19.254515
48.676434	1405.807291	19.259533
48.700034	1400.712550	19.264551
48.913611	1399.518975	19.269568
48.575987	1407.666934	19.274586
49.158252	1408.385121	19.279603
48.941902	1404.323402	19.284621
48.807020	1398.943882	19.289639
49.053371	1395.918923	19.294656
48.788352	1401.828904	19.299674
48.935979	1391.195203	19.304691
48.914716	1401.146261	19.309709
48.947389	1409.406134	19.314727
49.122959	1393.102133	19.319744
49.066783	1400.154289	19.324762
49.238428	1402.869572	19.329779
49.447251	1396.444968	19.334797
49.035046	1394.198727	19.339815
49.252188	1383.777533	19.344832
48.967277	1401.652444	19.349850
49.357347	1415.542830	19.354867
49.613445	1414.651265	19.359885
49.983950	1429.811029	19.364903
49.971339	1427.928141	19.369920
49.860538	1428.466994	19.374938
50.082291	1428.597245	19.379955
50.066055	1423.279566	19.384973
49.818127	1427.843044	19.389991
50.356921	1417.910688	19.395008
50.014083	1430.127581	19.400026
50.470884	1418.482838	19.405043
49.946677	1405.145442	19.410061
49.819703	1409.146374	19.415079
50.135589	1405.030781	19.420096
49.743273	1425.576223	19.425114
50.093560	1414.934146	19.430131
50.243823	1414.017980	19.435149
49.939651	1426.000124	19.440167
49.818454	1419.333307	19.445184
49.783832	1441.873457	19.450202
50.032354	1446.402770	19.455219
50.483738	1455.399235	19.460237
50.292752	1444.471174	19.465255
50.729555	1444.633533	19.470272
50.306541	1451.426377	19.475290
50.323478	1461.529021	19.480307
50.914529	1464.887463	19.485325
51.067565	1466.468055	19.490343
51.575623	1465.804451	19.495360
51.027353	1468.516507	19.500378
51.357039	1457.843954	19.505395
51.360634	1446.391946	19.510413
51.023368	1431.989727	19.515431
51.036527	1435.063537	19.520448
50.691890	1447.134285	19.525466
50.992826	1449.731714	19.530483
51.301024	1460.775491	19.535501
51.197201	1463.813165	19.540519
51.537816	1465.597735	19.545536
51.557867	1464.925171	19.550554
51.636620	1462.036610	19.555571
51.643589	1454.082034	19.560589
51.525523	1463.714913	19.565607
51.647327	1460.005058	19.570624
51.527331	1462.677697	19.575642
51.487007	1451.129808	19.580659
51.792799	1458.487408	19.585677
51.490649	1479.837670	19.590695
52.035095	1486.538450	19.595712
51.838589	1483.332866	19.600730
51.552909	1481.320777	19.605747
51.822236	1483.665573	19.610765
51.682361	1484.572625	19.615783
51.973446	1484.241007	19.620800
52.271529	1497.540797	19.625818
52.211442	1510.518016	19.630835
53.151989	1502.484428	19.635853
52.477820	1493.472542	19.640871
52.682100	1479.588087	19.645888
52.604500	1486.893828	19.650906
52.501912	1473.073574	19.655923
52.908006	1477.047284	19.660941
52.767306	1475.694255	19.665959
53.102690	1472.973435	19.670976
52.697304	1460.063557	19.675994
52.574658	1472.488903	19.681011
52.832589	1465.319927	19.686029
52.705523	1473.918878	19.691047
52.767555	1464.800073	19.696064
52.746280	1465.522133	19.701082
52.666514	1492.372152	19.706099
53.112585	1491.256217	19.711117
53.025612	1507.024870	19.716135
53.480413	1500.971697	19.721152
53.139418	1505.924226	19.726170
53.180715	1501.119039	19.731187
53.314661	1505.798442	19.736205
53.040605	1504.665128	19.741223
53.266240	1500.196739	19.746240
53.555877	1504.615326	19.751258
53.390786	1504.824590	19.756275
53.318427	1497.493359	19.761293
53.315608	1510.746527	19.766311
53.568010	1513.869322	19.771328
53.615434	1512.216639	19.776346
53.642379	1522.779868	19.781363
53.750270	1513.051476	19.786381
53.623171	1515.323334	19.791399
53.885990	1514.141283	19.796416
53.912837	1516.882924	19.801434
53.809075	1518.550922	19.806451
53.973716	1536.030689	19.811469
54.245730	1544.832104	19.816487
54.201354	1537.191498	19.821504
54.355054	1526.290558	19.826522
54.065939	1539.043519	19.831539
54.478494	1527.812318	19.836557
54.391685	1536.316451	19.841575
54.549833	1530.474983	19.846592
54.663739	1539.055331	19.851610
54.516732	1545.024172	19.856627
54.710476	1532.439440	19.861645
54.627849	1539.071632	19.866663
54.799658	1539.634167	19.871680
55.192840	1533.206541	19.876698
54.833350	1535.246803	19.881715
55.297876	1525.307779	19.886733
54.923146	1527.799379	19.891751
55.131897	1529.784530	19.896768
55.071888	1525.741774	19.901786
54.841111	1537.468938	19.906803
55.355812	1551.947470	19.911821
54.791928	1559.803444	19.916839
54.963877	1555.689597	19.921856
55.296317	1562.538506	19.926874
55.180736	1569.039552	19.931891
55.682741	1552.058896	19.936909
55.316546	1547.993997	19.941927
55.641948	1557.216893	19.946944
55.353848	1554.080790	19.951962
55.500800	1567.115901	19.956979
55.890439	1569.567562	19.961997
56.130751	1580.171879	19.967015
56.009337	1579.247537	19.972032
55.999285	1588.792923	19.977050
55.795558	1583.129463	19.982067
56.250784	1572.617935	19.987085
56.383006	1579.594096	19.992103
56.134760	1568.044721	19.997120
56.590205	1565.811878	20.002138
56.264004	1565.877346	20.007155
56.370376	1544.422457	20.012173
56.330432	1553.023169	20.017191
56.548691	1550.488263	20.022208
56.452768	1550.799066	20.027226
56.299101	1568.452046	20.032243
57.073412	1564.888852	20.037261
56.640660	1571.426274	20.042279
56.678771	1575.914480	20.047296
56.945478	1576.182171	20.052314
56.579354	1584.123130	20.057331
56.542988	1580.607546	20.062349
56.313286	1579.541291	20.067367
56.649129	1582.833355	20.072384
57.019589	1576.402781	20.077402
56.393849	1585.183180	20.082419
56.861091	1596.326312	20.087437
56.795708	1606.163547	20.092455
56.868209	1604.143317	20.097472
56.966768	1605.367589	20.102490
56.657074	1615.175597	20.107507
57.050578	1626.762062	20.112525
57.352263	1632.705070	20.117543
57.433013	1631.577960	20.122560
57.795241	1634.434563	20.127578
57.661810	1636.729534	20.132595
58.135160	1621.404337	20.137613
57.935618	1628.527578	20.142631
57.733775	1623.194107	20.147648
58.192408	1613.904822	20.152666
58.189532	1627.882509	20.157683
58.500930	1620.068781	20.162701
58.192249	1621.961271	20.167719
58.098699	1620.588218	20.172736
58.362137	1617.521805	20.177754
58.167832	1623.724886	20.182771
58.325175	1614.643754	20.187789
58.265168	1610.914361	20.192807
58.147647	1613.655120	20.197824
58.257674	1614.086549	20.202842
58.173272	1617.665132	20.207859
58.171558	1613.301677	20.212877
58.405749	1631.592477	20.217895
58.296949	1641.844798	20.222912
58.415702	1652.013779	20.227930
58.468367	1658.683857	20.232947
58.857887	1648.571741	20.237965
59.158465	1643.442083	20.242983
58.875184	1649.575260	20.248000
58.932968	1642.750366	20.253018
59.444426	1643.988166	20.258035
59.302029	1638.502326	20.263053
59.077392	1640.280114	20.268071
59.124076	1636.880294	20.273088
58.966296	1637.802524	20.278106
59.473296	1664.607656	20.283123
59.493730	1673.877967	20.288141
59.633788	1673.131587	20.293159
59.524050	1679.702579	20.298176
59.587090	1663.959055	20.303194
59.955265	1662.913880	20.308211
59.831202	1677.796326	20.313229
59.855357	1673.776210	20.318247
59.708660	1673.530066	20.323264
59.805887	1659.556089	20.328282
59.536887	1674.342844	20.333299
60.208619	1664.240684	20.338317
60.450557	1662.187274	20.343335
60.420982	1673.889495	20.348352
60.316277	1655.296971	20.353370
59.900550	1662.174132	20.358387
60.173630	1657.895481	20.363405
60.419321	1659.085948	20.368423
60.227681	1662.522453	20.373440
60.308392	1658.268173	20.378458
59.998926	1661.981669	20.383475
60.272187	1664.126629	20.388493
60.348552	1675.385325	20.393511
60.455751	1680.740078	20.398528
60.539582	1688.022334	20.403546
60.663044	1684.998770	20.408563
60.943678	1681.714142	20.413581
60.869724	1689.230004	20.418599
60.882532	1682.632619	20.423616
61.021793	1678.631632	20.428634
60.744464	1690.729220	20.433651
61.091528	1702.860049	20.438669
61.164188	1713.037489	20.443687
60.926528	1710.309147	20.448704
61.470454	1706.365168	20.453722
61.357894	1711.471277	20.458739
61.173698	1708.090378	20.463757
61.388753	1712.971377	20.468775
61.313624	1708.557058	20.473792
61.842019	1722.407889	20.478810
61.810669	1728.507652	20.483827
61.917202	1737.744454	20.488845
62.179404	1724.124996	20.493863
61.986609	1728.670377	20.498880
62.192019	1726.165130	20.503898
62.242074	1730.095100	20.508915
62.020832	1723.853381	20.513933
62.299722	1721.300141	20.518951
62.349522	1727.531350	20.523968
62.606166	1710.216736	20.528986
62.450180	1729.780136	20.534003
62.725762	1724.267973	20.539021
62.891365	1721.810657	20.544039
62.465041	1709.976090	20.549056
62.536449	1696.859903	20.554074
62.709955	1710.807279	20.559091
62.787476	1719.678400	20.564109
62.784178	1715.163603	20.569127
62.654614	1715.420924	20.574144
62.916797	1717.775208	20.579162
62.871312	1719.144994	20.584179
62.902535	1721.316257	20.589197
62.767445	1720.379210	20.594215
62.413779	1728.556763	20.599232
62.699687	1732.590991	20.604250
62.923726	1751.924174	20.609267
63.234953	1748.846673	20.614285
63.141777	1748.815684	20.619303
63.053337	1754.363487	20.624320
63.365061	1751.171336	20.629338
63.276746	1768.009384	20.634355
63.579307	1771.047548	20.639373
64.006570	1776.150126	20.644391
63.848520	1776.836579	20.649408
63.805258	1772.605944	20.654426
63.531236	1776.497458	20.659443
63.534556	1766.418501	20.664461
63.835916	1770.639947	20.669479
63.820856	1775.974425	20.674496
64.021913	1773.689185	20.679514
64.162869	1773.500925	20.684531
64.085245	1793.592381	20.689549
64.584378	1796.625563	20.694567
64.576121	1804.088083	20.699584
64.742667	1801.161301	20.704602
64.299315	1793.437020	20.709619
64.585151	1797.265763	20.714637
64.843700	1794.926118	20.719655
64.623333	1800.427277	20.724672
64.815363	1794.921442	20.729690
64.920181	1798.786457	20.734707
64.826946	1796.931047	20.739725
65.115094	1790.880553	20.744743
64.926772	1796.296482	20.749760
64.739194	1797.716574	20.754778
64.417037	1795.136853	20.759795
64.701003	1802.117912	20.764813
65.073239	1813.112757	20.769831
65.246727	1821.032601	20.774848
65.124170	1816.091058	20.779866
65.459413	1817.447421	20.784883
65.427789	1824.281922	20.789901
65.862562	1810.997993	20.794919
65.557920	1820.462375	20.799936
65.659579	1816.041196	20.804954
65.824031	1804.170159	20.809971
65.501086	1821.914840	20.814989
66.103472	1831.458974	20.820007
66.205513	1846.867538	20.825024
66.031444	1845.036530	20.830042
66.256517	1849.735596	20.835059
66.090536	1854.144681	20.840077
66.235805	1848.380425	20.845095
66.318009	1848.246381	20.850112
66.481366	1844.731527	20.855130
66.728392	1848.057646	20.860147
66.154978	1849.888482	20.865165
66.307356	1842.281290	20.870183
66.719996	1845.315417	20.875200
66.792845	1838.947792	20.880218
66.934584	1835.982984	20.885235
66.994514	1839.940088	20.890253
66.778434	1837.985719	20.895271
66.498452	1842.927070	20.900288
66.781391	1856.891499	20.905306
67.320670	1856.508938	20.910323
67.025889	1863.464588	20.915341
67.339385	1857.598458	20.920359
67.203685	1862.682464	20.925376
67.381816	1854.960371	20.930394
67.381043	1850.127788	20.935411
67.422698	1853.713507	20.940429
67.403692	1853.228498	20.945447
67.657717	1864.765794	20.950464
67.339960	1880.064368	20.955482
67.576078	1879.830035	20.960499
67.631767	1883.837854	20.965517
67.741094	1880.873285	20.970535
67.887118	1882.259803	20.975552
67.878860	1875.054790	20.980570
67.968769	1868.986694	20.985587
67.844553	1884.732370	20.990605
68.187834	1899.748282	20.995623
68.608460	1902.807870	21.000640
68.459129	1907.177205	21.005658
68.639614	1902.906339	21.010675
68.461894	1905.327975	21.015693
68.594183	1901.696203	21.020711
68.741683	1900.526919	21.025728
68.687574	1896.464585	21.030746
68.797832	1897.513712	21.035763
68.719303	1895.056238	21.040781
68.962151	1902.804007	21.045799
68.686973	1902.693701	21.050816
68.950675	1898.615361	21.055834
69.238533	1888.232122	21.060851
69.169581	1894.861020	21.065869
69.368159	1892.516330	21.070887
69.099907	1887.013443	21.075904
68.993720	1892.660299	21.080922
69.372327	1906.771141	21.085939
69.310725	1927.774308	21.090957
69.225816	1920.314637	21.095975
69.595581	1921.675924	21.100992
69.481108	1927.120617	21.106010
69.643872	1923.234970	21.111027
69.329786	1934.241960	21.116045
69.864973	1935.926260	21.121063
69.581868	1944.955646	21.126080
69.700383	1954.858718	21.131098
70.070007	1942.722498	21.136115
70.054277	1950.028842	21.141133
70.039989	1943.988206	21.146151
70.427685	1946.564269	21.151168
70.342590	1938.429015	21.156186
70.577846	1969.800631	21.161203
70.494366	1968.465250	21.166221
70.714380	1974.461284	21.171239
71.093926	1966.110105	21.176256
71.085633	1965.335911	21.181274
71.307963	1957.618260	21.186291
71.419117	1950.934004	21.191309
71.438097	1930.521420	21.196327
71.248881	1929.948446	21.201344
71.200488	1921.370501	21.206362
71.529973	1915.206421	21.211379
71.258016	1924.560727	21.216397
71.463792	1918.647448	21.221415
71.257288	1925.452286	21.226432
71.272477	1923.858048	21.231450
71.390000	1928.570221	21.236467
71.715621	1960.151664	21.241485
71.847380	1952.222629	21.246503
71.798137	1960.877469	21.251520
71.901902	1959.011470	21.256538
72.209443	1953.251804	21.261555
71.986023	1956.348746	21.266573
72.265812	1955.967021	21.271591
71.835841	1954.405146	21.276608
71.940409	1952.596496	21.281626
72.146810	1943.506263	21.286643
72.164233	1955.746990	21.291661
72.044212	1949.506137	21.296679
72.102109	1953.358880	21.301696
72.208077	1976.536385	21.306714
72.386337	1974.685609	21.311731
72.393195	1983.482752	21.316749
72.509762	1983.585936	21.321767
72.664732	1979.394866	21.326784
72.445626	1993.811055	21.331802
72.680022	2005.763528	21.336819
72.667080	2022.237788	21.341837
72.905141	2008.866573	21.346855
73.151059	2015.799304	21.351872
72.742644	2012.505463	21.356890
73.215978	2003.965108	21.361907
73.256604	2016.447322	21.366925
73.602528	2022.055590	21.371943
73.821298	2030.579871	21.376960
73.758251	2031.448248	21.381978
74.059093	2019.581237	21.386995
73.818772	2011.926775	21.392013
73.800723	1994.364799	21.397031
74.004094	2002.941222	21.402048
74.123856	2010.005077	21.407066
74.204318	2011.877670	21.412083
74.212361	2026.532666	21.417101
74.435577	2022.582260	21.422119
74.387145	2019.164246	21.427136
74.431030	2021.287784	21.432154
74.375944	2019.022871	21.437171
74.586423	2019.063261	21.442189
74.295016	2020.887187	21.447207
74.620783	2016.858778	21.452224
74.716481	2028.811792	21.457242
74.699030	2021.505080	21.462259
74.424274	2029.989418	21.467277
74.427090	2023.544334	21.472295
74.847226	2022.586600	21.477312
74.848120	2041.694879	21.482330
74.829054	2040.022440	21.487347
74.767702	2051.715640	21.492365
74.826595	2047.045563	21.497383
75.077495	2049.622640	21.502400
75.244550	2066.349041	21.507418
75.215202	2072.283248	21.512435
75.101269	2078.818488	21.517453
74.966058	2083.470188	21.522471
75.270212	2084.765186	21.527488
75.646832	2101.272670	21.532506
76.313401	2091.117154	21.537523
76.387372	2103.782900	21.542541
76.547713	2096.243954	21.547559
76.671124	2088.532381	21.552576
76.924235	2089.677558	21.557594
76.691988	2072.973424	21.562611
76.445576	2064.338025	21.567629
76.091035	2067.739778	21.572647
76.623393	2065.452793	21.577664
76.581236	2066.557877	21.582682
76.663350	2082.511724	21.587699
76.675767	2092.134016	21.592717
76.375778	2090.373041	21.597735
76.901366	2082.718508	21.602752
76.646266	2106.698925	21.607770
76.638418	2093.450640	21.612787
76.913943	2100.178106	21.617805
76.920110	2108.109659	21.622823
77.438248	2116.528121	21.627840
77.225364	2126.612161	21.632858
77.119302	2126.002577	21.637875
77.031953	2126.379296	21.642893
77.114379	2119.219393	21.647911
77.650566	2115.280927	21.652928
77.349400	2136.028756	21.657946
77.575675	2152.005262	21.662963
78.112493	2151.577828	21.667981
77.967386	2155.275250	21.672999
78.358495	2151.113936	21.678016
78.338814	2155.794957	21.683034
78.375590	2142.541209	21.688051
78.323158	2134.658327	21.693069
78.316474	2141.651442	21.698087
78.529032	2132.171484	21.703104
78.106276	2150.268115	21.708122
78.067683	2136.724085	21.713139
78.266196	2142.465075	21.718157
78.330995	2143.518596	21.723175
78.754731	2147.643898	21.728192
78.711554	2166.238349	21.733210
78.935438	2163.517368	21.738227
79.253020	2167.120075	21.743245
78.863776	2166.647142	21.748263
79.365458	2161.102509	21.753280
79.132817	2173.373392	21.758298
79.478344	2165.887613	21.763315
79.349683	2151.044263	21.768333
79.012501	2162.895818	21.773351
79.288308	2164.418753	21.778368
79.480423	2173.795981	21.783386
79.650474	2185.034024	21.788403
79.746719	2186.596928	21.793421
79.943714	2190.176296	21.798439
80.244798	2189.757969	21.803456
79.885849	2195.042832	21.808474
79.940657	2185.401946	21.813491
79.834570	2188.655497	21.818509
79.823788	2183.041762	21.823527
80.103348	2187.809473	21.828544
80.228102	2199.432992	21.833562
80.187189	2199.609104	21.838579
80.175212	2208.243345	21.843597
80.099391	2205.820020	21.848615
80.865176	2213.109302	21.853632
80.697024	2239.283092	21.858650
80.765026	2235.803231	21.863667
81.020529	2240.348160	21.868685
80.897922	2233.551299	21.873703
81.276805	2230.383761	21.878720
81.217517	2230.336529	21.883738
80.790422	2227.570951	21.888755
81.488435	2236.455386	21.893773
81.343153	2259.230013	21.898791
81.480070	2244.774116	21.903808
81.645538	2256.580315	21.908826
81.722181	2254.358520	21.913843
81.862321	2252.558513	21.918861
81.930086	2262.833193	21.923879
81.983087	2253.379186	21.928896
81.776091	2254.534017	21.933914
81.914197	2254.539539	21.938931
82.069567	2262.830735	21.943949
82.211490	2272.682102	21.948967
82.793879	2271.476615	21.953984
82.784455	2284.533891	21.959002
82.539545	2278.391933	21.964019
82.832785	2281.574663	21.969037
82.909329	2275.357828	21.974055
83.297586	2270.431963	21.979072
83.083251	2257.510257	21.984090
83.188373	2248.495280	21.989107
83.147606	2238.880421	21.994125
83.016874	2240.564773	21.999143
83.274597	2248.450023	22.004160
82.904075	2257.546426	22.009178
83.585360	2258.622693	22.014195
83.722604	2257.067270	22.019213
83.361329	2262.995480	22.024231
83.377477	2262.819612	22.029248
83.477224	2268.647083	22.034266
83.788162	2270.848099	22.039283
83.635109	2269.675793	22.044301
83.548900	2260.666108	22.049319
83.775228	2259.673518	22.054336
83.940167	2273.241308	22.059354
83.689091	2288.558770	22.064371
83.750235	2283.670917	22.069389
84.029080	2288.575004	22.074407
84.000163	2285.562379	22.079424
84.257440	2305.926228	22.084442
84.179876	2318.259742	22.089459
84.484260	2323.376550	22.094477
84.110603	2327.014998	22.099495
84.586138	2320.927370	22.104512
84.605806	2339.975030	22.109530
84.592171	2354.309893	22.114547
84.854940	2345.623499	22.119565
85.153077	2346.495481	22.124583
85.561356	2347.597270	22.129600
85.573320	2341.005258	22.134618
85.270786	2347.858857	22.139635
85.570230	2337.821844	22.144653
85.332761	2337.940733	22.149671
85.837315	2346.571029	22.154688
86.088260	2357.078053	22.159706
85.994986	2338.997408	22.164723
86.124128	2345.575195	22.169741
85.931074	2348.878613	22.174759
86.047518	2353.008783	22.179776
86.185555	2367.476821	22.184794
86.346815	2371.633830	22.189811
86.427401	2362.483472	22.194829
86.092494	2371.186625	22.199847
86.484894	2364.778870	22.204864
86.419305	2363.432225	22.209882
86.262729	2364.723211	22.214899
86.237487	2372.725850	22.219917
86.576018	2396.910804	22.224935
86.845422	2389.019392	22.229952
87.155918	2402.743125	22.234970
86.895902	2403.533892	22.239987
87.427197	2389.833472	22.245005
87.305043	2400.201501	22.250023
87.527416	2410.630216	22.255040
87.481293	2410.405204	22.260058
87.513087	2419.691404	22.265075
87.799465	2411.916466	22.270093
87.565471	2424.624407	22.275111
87.681408	2412.941264	22.280128
87.857276	2414.102799	22.285146
87.876721	2414.992186	22.290163
88.099799	2408.407319	22.295181
87.987016	2417.014269	22.300199
87.974816	2427.898390	22.305216
88.070238	2427.526708	22.310234
88.022190	2442.016963	22.315251
88.598467	2433.520360	22.320269
88.838134	2436.883655	22.325287
88.809121	2429.868445	22.330304
88.696043	2432.542859	22.335322
88.662789	2433.868160	22.340339
88.924556	2440.423241	22.345357
88.979564	2460.781410	22.350375
88.783158	2461.822291	22.355392
89.424746	2465.676952	22.360410
89.275150	2465.956106	22.365427
89.603482	2455.851239	22.370445
89.817575	2461.289752	22.375463
89.542707	2467.036794	22.380480
89.567145	2458.766984	22.385498
89.487515	2459.237714	22.390515
89.999158	2461.610657	22.395533
89.857135	2458.387973	22.400551
90.069093	2460.045532	22.405568
90.124515	2457.133483	22.410586
89.722742	2455.195212	22.415603
89.987418	2457.025942	22.420621
90.307699	2473.473069	22.425639
90.101461	2479.204028	22.430656
90.388504	2471.383673	22.435674
90.379511	2471.987598	22.440691
90.732146	2472.265887	22.445709
90.275326	2478.463161	22.450727
90.663314	2493.743523	22.455744
90.757030	2504.568821	22.460762
90.950648	2511.371843	22.465779
91.390865	2498.229748	22.470797
91.185364	2503.798380	22.475815
90.937049	2501.521290	22.480832
91.328538	2512.457144	22.485850
91.202455	2528.136058	22.490867
91.996776	2524.159873	22.495885
92.134474	2529.261825	22.500903
92.102456	2535.730146	22.505920
92.208507	2528.185807	22.510938
91.952866	2526.163092	22.515955
92.369373	2524.391317	22.520973
92.038833	2534.114369	22.525991
92.238819	2535.097894	22.531008
92.334002	2528.711722	22.536026
92.080738	2524.362886	22.541043
92.431790	2514.925125	22.546061
92.295678	2520.602754	22.551079
92.667959	2539.278874	22.556096
92.948424	2546.534883	22.561114
93.073117	2554.760051	22.566131
92.974280	2563.599432	22.571149
92.811913	2548.460083	22.576167
92.917530	2560.072473	22.581184
92.861601	2548.232240	22.586202
92.940237	2568.832322	22.591219
93.660100	2565.099177	22.596237
93.671518	2575.919646	22.601255
93.637240	2572.734220	22.606272
93.457448	2579.849899	22.611290
93.521366	2584.160098	22.616307
93.632580	2576.448335	22.621325
93.644640	2587.571480	22.626343
93.742049	2594.080212	22.631360
94.332470	2602.932671	22.636378
94.050976	2613.764258	22.641395
93.581104	2595.390920	22.646413
93.799327	2607.336299	22.651431
94.183466	2627.187408	22.656448
94.590060	2622.264697	22.661466
94.860296	2631.948188	22.666483
94.758545	2622.876689	22.671501
95.068511	2635.353785	22.676519
95.226518	2650.990511	22.681536
95.803532	2642.688962	22.686554
95.546033	2630.237902	22.691571
95.331290	2611.369519	22.696589
95.341470	2616.091800	22.701607
95.566397	2629.843289	22.706624
95.505763	2633.900877	22.711642
95.765489	2646.913107	22.716659
96.085922	2641.939297	22.721677
95.936570	2633.228452	22.726695
95.924939	2643.250369	22.731712
96.089108	2641.419173	22.736730
95.697226	2655.090117	22.741747
96.092248	2646.337564	22.746765
95.798277	2650.555844	22.751783
95.590113	2659.353140	22.756800
95.775721	2660.280389	22.761818
95.808277	2678.462098	22.766835
96.010331	2694.817609	22.771853
96.412050	2703.826181	22.776871
96.353844	2706.436828	22.781888
96.795302	2709.136808	22.786906
96.559566	2730.684885	22.791923
97.590835	2733.399037	22.796941
97.449797	2723.410295	22.801959
97.265087	2728.243622	22.806976
97.624245	2724.082331	22.811994
97.326156	2737.086197	22.817011
97.232009	2727.014881	22.822029
98.041859	2740.696792	22.827047
97.944071	2748.102930	22.832064
98.496548	2748.128044	22.837082
98.208723	2751.477947	22.842099
98.461678	2745.094701	22.847117
98.648466	2745.196897	22.852135
98.368281	2749.090456	22.857152
98.628446	2756.821220	22.862170
98.454109	2749.284611	22.867187
98.629739	2749.068552	22.872205
98.767792	2740.087605	22.877223
98.625733	2751.100153	22.882240
98.956727	2747.356148	22.887258
98.729994	2748.241821	22.892275
99.002833	2760.849978	22.897293
99.059048	2774.920100	22.902311
99.125837	2782.538787	22.907328
99.060249	2775.760597	22.912346
99.005143	2781.964319	22.917363
99.437688	2798.020341	22.922381
99.816392	2801.088628	22.927399
99.549646	2803.435370	22.932416
99.864513	2800.047593	22.937434
99.867821	2793.175698	22.942451
100.066940	2807.129270	22.947469
100.720100	2820.465907	22.952487
100.341080	2827.071727	22.957504
100.723716	2818.444367	22.962522
100.581439	2821.493395	22.967539
100.640349	2818.405097	22.972557
100.986604	2811.795731	22.977575
100.740835	2815.048520	22.982592
100.895398	2803.700055	22.987610
101.250301	2813.969688	22.992627
100.921303	2816.067664	22.997645
101.303816	2813.846727	23.002663
101.120020	2818.406288	23.007680
101.194638	2838.561294	23.012698
101.162630	2844.054468	23.017715
101.282186	2842.370016	23.022733
101.349588	2851.611598	23.027751
101.689232	2863.474468	23.032768
101.925044	2868.721718	23.037786
101.501374	2879.822717	23.042803
101.908760	2872.292500	23.047821
102.106064	2865.077012	23.052839
102.205190	2872.659678	23.057856
102.304325	2868.268938	23.062874
102.608164	2871.074022	23.067891
102.267331	2891.895961	23.072909
102.675306	2891.927676	23.077927
102.638336	2891.701535	23.082944
103.091420	2887.656552	23.087962
103.282998	2889.756938	23.092979
103.231770	2886.576224	23.097997
103.586999	2883.761321	23.103015
103.500004	2890.756650	23.108032
103.642969	2883.109564	23.113050
103.467535	2880.736486	23.118067
103.456722	2890.953324	23.123085
103.722656	2894.100149	23.128103
103.855510	2899.700704	23.133120
103.884275	2898.271849	23.138138
104.019363	2909.577627	23.143155
103.672205	2919.885213	23.148173
104.116184	2908.269839	23.153191
103.988113	2909.244706	23.158208
104.536392	2935.595956	23.163226
104.527458	2937.066105	23.168243
104.431967	2943.856547	23.173261
104.670487	2935.755782	23.178279
104.482164	2946.849362	23.183296
104.891311	2944.157029	23.188314
104.774415	2959.298194	23.193331
104.799697	2960.755199	23.198349
105.072737	2959.039418	23.203367
104.793488	2971.226902	23.208384
104.943559	2980.563544	23.213402
105.232066	2990.339912	23.218419
105.470657	2993.456635	23.223437
105.586436	3001.325609	23.228455
105.632272	3022.674307	23.233472
105.723531	3008.848941	23.238490
106.061881	3014.552535	23.243507
106.333391	3009.417404	23.248525
106.837128	3002.319639	23.253543
106.896311	3015.405935	23.258560
106.595181	3011.622022	23.263578
106.791609	3006.063457	23.268595
106.821429	3019.462913	23.273613
106.952280	3028.580699	23.278631
106.988640	3038.611067	23.283648
107.694653	3032.192857	23.288666
107.392062	3029.823484	23.293683
107.175386	3025.820055	23.298701
107.490186	3027.819344	23.303719
107.109163	3037.756595	23.308736
107.300195	3027.613851	23.313754
107.642939	3045.005195	23.318771
107.806824	3044.897781	23.323789
108.101609	3039.587117	23.328807
108.050536	3046.693902	23.333824
108.027214	3045.085451	23.338842
108.647128	3037.875120	23.343859
108.494477	3039.089125	23.348877
108.515629	3043.775463	23.353895
108.429824	3049.442198	23.358912
108.550519	3064.858725	23.363930
108.623873	3073.380095	23.368947
108.804374	3078.081010	23.373965
109.300316	3078.976199	23.378983
109.292183	3078.594085	23.384000
109.094320	3070.962387	23.389018
109.343224	3072.177242	23.394035
109.011220	3075.934171	23.399053
109.375265	3074.930544	23.404071
109.760793	3093.529147	23.409088
110.045388	3098.399860	23.414106
110.154573	3101.753798	23.419123
109.803321	3101.500152	23.424141
110.019599	3099.360642	23.429159
110.112207	3094.658290	23.434176
110.076772	3096.410426	23.439194
110.414837	3093.310900	23.444211
110.118206	3101.838024	23.449229
110.414815	3116.258062	23.454247
110.555809	3126.117999	23.459264
110.635118	3132.795323	23.464282
110.956765	3124.588169	23.469299
110.870420	3126.447173	23.474317
110.960422	3145.629856	23.479335
110.726632	3156.226731	23.484352
111.135261	3156.574908	23.489370
111.125824	3150.353849	23.494387
111.143184	3172.747333	23.499405
111.675574	3174.406650	23.504423
111.745592	3178.735691	23.509440
111.609181	3176.710079	23.514458
112.171765	3180.627616	23.519475
112.065908	3195.145072	23.524493
112.398073	3202.742865	23.529511
112.438433	3209.744813	23.534528
112.484400	3210.005775	23.539546
112.876867	3201.994752	23.544563
112.859150	3202.098917	23.549581
112.933506	3189.807842	23.554599
112.909184	3194.656889	23.559616
113.147142	3214.538463	23.564634
113.314036	3213.867499	23.569651
113.187904	3230.873639	23.574669
113.429920	3216.537254	23.579687
113.440297	3224.313149	23.584704
113.292727	3225.955112	23.589722
113.771572	3217.530132	23.594739
113.514619	3238.177997	23.599757
114.069991	3244.899793	23.604775
114.075120	3251.694972	23.609792
114.063093	3258.169733	23.614810
114.081332	3249.408746	23.619827
114.213822	3257.645988	23.624845
114.301732	3273.780035	23.629863
114.826870	3287.560364	23.634880
114.576169	3283.262863	23.639898
114.453709	3270.940917	23.644915
114.901497	3280.548956	23.649933
114.954119	3289.706227	23.654951
115.314650	3298.353422	23.659968
115.525271	3300.809806	23.664986
115.822175	3290.873011	23.670003
115.608114	3303.147214	23.675021
115.697892	3296.517109	23.680039
116.013566	3291.793911	23.685056
116.050701	3291.562976	23.690074
116.290165	3284.767527	23.695091
115.986948	3298.952361	23.700109
115.983317	3311.844165	23.705127
116.452276	3311.710653	23.710144
116.314423	3324.942441	23.715162
116.478236	3325.435103	23.720179
116.591891	3332.389534	23.725197
116.752683	3327.731342	23.730215
116.625780	3329.156091	23.735232
116.902367	3347.293846	23.740250
117.416049	3336.977787	23.745267
117.184035	3344.073714	23.750285
117.166335	3342.875764	23.755303
117.391345	3333.101649	23.760320
117.379818	3345.198637	23.765338
117.823432	3353.487581	23.770355
117.720869	3376.087059	23.775373
117.996769	3368.953614	23.780391
118.411820	3361.830604	23.785408
118.263887	3371.990921	23.790426
118.372826	3367.751191	23.795443
118.083964	3371.504591	23.800461
118.362705	3379.685003	23.805479
118.789121	3382.137567	23.810496
118.721675	3384.702213	23.815514
118.888006	3379.629262	23.820531
118.899805	3386.207623	23.825549
119.150696	3378.851124	23.830567
119.362358	3378.621612	23.835584
119.600787	3406.256594	23.840602
119.700866	3404.595782	23.845619
119.460204	3402.781124	23.850637
119.964944	3407.140236	23.855655
120.110345	3412.569588	23.860672
120.096336	3412.317588	23.865690
120.280135	3397.845777	23.870707
120.027806	3414.344208	23.875725
120.388956	3400.698643	23.880743
120.414273	3416.460480	23.885760
120.459589	3437.327885	23.890778
120.694722	3438.380858	23.895795
120.726438	3438.865862	23.900813
120.644845	3434.314705	23.905831
120.580547	3432.585030	23.910848
120.559772	3461.723825	23.915866
121.102963	3461.100801	23.920883
121.487452	3471.746726	23.925901
121.546254	3487.652321	23.930919
121.609946	3492.640056	23.935936
121.355527	3494.438335	23.940954
121.835955	3492.101871	23.945971
121.854741	3493.517477	23.950989
122.154583	3507.855443	23.956007
122.319136	3512.659143	23.961024
122.351788	3517.307888	23.966042
122.339367	3515.288479	23.971059
122.629773	3518.564468	23.976077
122.738754	3513.147776	23.981095
123.105144	3531.446097	23.986112
122.993140	3540.273246	23.991130
123.544915	3546.592177	23.996147
123.757835	3542.869503	24.001165
123.594985	3546.756038	24.006183
123.689130	3544.839863	24.011200
123.584586	3546.191629	24.016218
123.802788	3546.427232	24.021235
123.883943	3546.010243	24.026253
123.919532	3544.775500	24.031271
124.087435	3542.113165	24.036288
124.219841	3562.292613	24.041306
124.262911	3566.469117	24.046323
124.647760	3567.648512	24.051341
124.533988	3556.346684	24.056359
124.637393	3560.815991	24.061376
124.461442	3566.846699	24.066394
124.832132	3574.010291	24.071411
124.746020	3596.238419	24.076429
124.812414	3586.448275	24.081447
125.120735	3585.236888	24.086464
124.923868	3611.633505	24.091482
125.711369	3605.153931	24.096499
125.740139	3616.643200	24.101517
125.550967	3614.951504	24.106535
125.748850	3618.226295	24.111552
125.702156	3620.763525	24.116570
125.877985	3633.847565	24.121587
126.177396	3634.495370	24.126605
126.133654	3658.238815	24.131623
126.367316	3647.336941	24.136640
126.396008	3668.354670	24.141658
126.542385	3658.756779	24.146675
126.966008	3672.809408	24.151693
127.115998	3674.963645	24.156711
127.416125	3666.075825	24.161728
127.361099	3689.053367	24.166746
127.255662	3690.797078	24.171763
127.480396	3695.976749	24.176781
127.738587	3698.154419	24.181799
128.187129	3691.523420	24.186816
127.895483	3698.672299	24.191834
128.248062	3694.211018	24.196851
128.334455	3705.638836	24.201869
128.405043	3716.610950	24.206887
128.333118	3718.458579	24.211904
128.537350	3729.662153	24.216922
128.621392	3711.797052	24.221939
128.816331	3727.032627	24.226957
128.926777	3731.366547	24.231975
128.970337	3740.863424	24.236992
129.039170	3741.893550	24.242010
129.198100	3735.769204	24.247027
129.496997	3746.135747	24.252045
129.148450	3758.309325	24.257063
129.947448	3768.572612	24.262080
129.968896	3775.367286	24.267098
129.661550	3769.294923	24.272115
129.693664	3772.368812	24.277133
129.760250	3792.116873	24.282151
130.303533	3787.890172	24.287168
130.361374	3807.809016	24.292186
130.544436	3816.960751	24.297203
130.820491	3815.844466	24.302221
130.826360	3823.275687	24.307239
131.204768	3819.243227	24.312256
131.114688	3829.297004	24.317274
131.268531	3842.047803	24.322291
131.587564	3845.836519	24.327309
131.536404	3844.930726	24.332327
131.888057	3842.839975	24.337344
132.147470	3846.048714	24.342362
131.806558	3839.786969	24.347379
131.959442	3842.507367	24.352397
132.075991	3858.172642	24.357415
132.311705	3866.663234	24.362432
132.591686	3864.229176	24.367450
132.534457	3864.382807	24.372467
132.940815	3870.326282	24.377485
132.747343	3879.922337	24.382503
133.101519	3882.147932	24.387520
133.262068	3886.813808	24.392538
133.301223	3889.908211	24.397555
133.619010	3892.241028	24.402573
133.546177	3884.455928	24.407591
133.593301	3883.611037	24.412608
133.558252	3894.659435	24.417626
133.779449	3914.463561	24.422643
134.010464	3925.771126	24.427661
133.862207	3926.991952	24.432679
133.813633	3922.804138	24.437696
134.006644	3941.609667	24.442714
134.993085	3942.731628	24.447731
134.780023	3938.621442	24.452749
134.899248	3945.450010	24.457767
135.376901	3936.530285	24.462784
135.389758	3943.581216	24.467802
135.237301	3937.923760	24.472819
135.450934	3937.289918	24.477837
135.386618	3958.390374	24.482855
135.858906	3964.938418	24.487872
135.396440	3972.486228	24.492890
135.238019	3970.442893	24.497907
135.807629	3969.739090	24.502925
136.055948	3995.188501	24.507943
136.159921	3994.182989	24.512960
136.493195	3990.284749	24.517978
136.665210	4001.669864	24.522995
136.527943	4019.730832	24.528013
136.459466	4026.238487	24.533031
136.872049	4027.390096	24.538048
137.072441	4033.742201	24.543066
137.074807	4053.659122	24.548083
137.296374	4057.915278	24.553101
137.460763	4061.394952	24.558119
137.196136	4056.612850	24.563136
137.521239	4076.264525	24.568154
137.600524	4075.341848	24.573171
138.048501	4091.936501	24.578189
138.118027	4114.255361	24.583207
138.307346	4112.343444	24.588224
138.476862	4111.725562	24.593242
138.638626	4113.123459	24.598259
139.366464	4112.917950	24.603277
138.884011	4125.054127	24.608295
139.122661	4128.632563	24.613312
139.481426	4144.981370	24.618330
139.537318	4152.705696	24.623347
139.448116	4122.822761	24.628365
139.377428	4132.359659	24.633383
139.802394	4140.281186	24.638400
139.910551	4154.155338	24.643418
140.000630	4150.916320	24.648435
140.264511	4145.459985	24.653453
140.323007	4159.129729	24.658471
140.508028	4163.254935	24.663488
140.603079	4172.422631	24.668506
140.386663	4177.052166	24.673523
140.895663	4178.561902	24.678541
140.692049	4185.806286	24.683559
141.173388	4198.443699	24.688576
141.552569	4199.656766	24.693594
141.346599	4197.389738	24.698611
141.668309	4201.140297	24.703629
141.442677	4218.294710	24.708647
141.834186	4223.800943	24.713664
141.980524	4224.011441	24.718682
142.229803	4233.983700	24.723699
142.312650	4223.838408	24.728717
142.523445	4233.101957	24.733735
142.401414	4249.286336	24.738752
142.843742	4258.350912	24.743770
142.897761	4262.056025	24.748787
143.009000	4259.778999	24.753805
142.991548	4262.666670	24.758823
142.572971	4258.239970	24.763840
143.354246	4271.208953	24.768858
143.335576	4282.641592	24.773875
143.511954	4285.672010	24.778893
143.632109	4288.230553	24.783911
143.813593	4303.941833	24.788928
144.045254	4307.593133	24.793946
143.849802	4317.619384	24.798963
144.140947	4316.322977	24.803981
144.114616	4347.180774	24.808999
143.977571	4349.903188	24.814016
144.450853	4361.363908	24.819034
144.432371	4375.702606	24.824051
145.074956	4371.034041	24.829069
145.035585	4374.431750	24.834087
145.189061	4393.660976	24.839104
145.590245	4399.195596	24.844122
145.716623	4392.964160	24.849139
145.931151	4395.621290	24.854157
145.950484	4409.930133	24.859175
146.342323	4411.282092	24.864192
146.771330	4426.029516	24.869210
146.432396	4432.836491	24.874227
146.778652	4422.860100	24.879245
146.633880	4416.549900	24.884263
146.953887	4434.380494	24.889280
147.260001	4429.396684	24.894298
147.305055	4455.301829	24.899315
147.658751	4452.876742	24.904333
147.435733	4452.979858	24.909351
147.382114	4447.019189	24.914368
147.932648	4448.960739	24.919386
147.514520	4459.626416	24.924403
147.814078	4469.681069	24.929421
147.944764	4475.429820	24.934439
147.799983	4487.155976	24.939456
148.428045	4492.707411	24.944474
148.532958	4509.272673	24.949491
149.044750	4505.792868	24.954509
148.884977	4508.330061	24.959527
149.167821	4517.551924	24.964544
149.105380	4533.888965	24.969562
149.195384	4535.876054	24.974579
149.465948	4529.727801	24.979597
149.794628	4544.316323	24.984615
149.999646	4561.549448	24.989632
150.362055	4563.638715	24.994650
150.091543	4563.753632	24.999667
150.391123	4554.001461	25.004685
150.359712	4558.416981	25.009703
150.858235	4568.351340	25.014720
150.781043	4566.520505	25.019738
150.601187	4569.175227	25.024755
150.816157	4572.606476	25.029773
151.101450	4586.737566	25.034791
151.100282	4598.610140	25.039808
151.502764	4602.200941	25.044826
151.285602	4614.638521	25.049843
151.706245	4616.715004	25.054861
151.737136	4629.784101	25.059879
151.956487	4629.291834	25.064896
151.984723	4641.439942	25.069914
152.302234	4653.498429	25.074931
152.680723	4652.766389	25.079949
152.945529	4668.590249	25.084967
152.835050	4665.029928	25.089984
152.803007	4659.714551	25.095002
153.144199	4666.203478	25.100019
153.246518	4680.323203	25.105037
153.355141	4677.870926	25.110055
153.316313	4685.867151	25.115072
153.647252	4680.934282	25.120090
153.849412	4707.131217	25.125107
153.703669	4709.939401	25.130125
153.690825	4710.948854	25.135143
153.804959	4718.493704	25.140160
154.325993	4733.259261	25.145178
154.481828	4745.897451	25.150195
154.463606	4742.612449	25.155213
154.626688	4760.541061	25.160231
154.684202	4774.272146	25.165248
155.037424	4768.442467	25.170266
155.074353	4789.114593	25.175283
155.502101	4793.202932	25.180301
155.592706	4802.578861	25.185319
155.126010	4807.201973	25.190336
156.099413	4814.389612	25.195354
155.976144	4823.821436	25.200371
156.378502	4808.794324	25.205389
156.307491	4836.996155	25.210407
156.377949	4850.577889	25.215424
156.939483	4854.244013	25.220442
157.028561	4863.542262	25.225459
157.203852	4871.591341	25.230477
157.580977	4880.602493	25.235495
157.465138	4885.635357	25.240512
157.796111	4880.981219	25.245530
157.719485	4885.786285	25.250547
157.912826	4887.863421	25.255565
158.125673	4896.760805	25.260583
158.054009	4907.925447	25.265600
158.588030	4898.726504	25.270618
158.286351	4908.076868	25.275635
158.490849	4920.849693	25.280653
159.055941	4926.792892	25.285671
159.013342	4938.267772	25.290688
159.000334	4942.715793	25.295706
159.168744	4952.738913	25.300723
159.776995	4962.049718	25.305741
159.841644	4963.696103	25.310759
159.658261	4972.956040	25.315776
160.013732	4976.657095	25.320794
159.933819	4988.672949	25.325811
160.079388	4990.711541	25.330829
160.316890	4996.873602	25.335847
160.702535	5012.447833	25.340864
161.039773	5007.405135	25.345882
161.073410	5012.329811	25.350899
160.975759	5011.497015	25.355917
161.369266	5018.671279	25.360935
161.260562	5035.225205	25.365952
161.769038	5035.712846	25.370970
161.604584	5037.826395	25.375987
161.606141	5043.019441	25.381005
161.448071	5048.381466	25.386023
162.091828	5064.529689	25.391040
162.202334	5072.316308	25.396058
162.136990	5101.500568	25.401075
161.975930	5094.642275	25.406093
162.734617	5106.559555	25.411111
162.615407	5117.652672	25.416128
163.146596	5121.382165	25.421146
163.153182	5139.693890	25.426163
163.359509	5151.779831	25.431181
163.727162	5154.582646	25.436199
163.976518	5155.715688	25.441216
164.679057	5152.053740	25.446234
164.621955	5151.200047	25.451251
164.542058	5153.138946	25.456269
164.461750	5140.543925	25.461287
164.358980	5157.037140	25.466304
165.190166	5163.938181	25.471322
165.200423	5169.030593	25.476339
165.400202	5174.928043	25.481357
165.326851	5175.243445	25.486375
165.160222	5180.168249	25.491392
165.506023	5203.802283	25.496410
165.696065	5207.703261	25.501427
165.871565	5210.823003	25.506445
165.935949	5209.364808	25.511463
166.244320	5233.239783	25.516480
166.209106	5232.884153	25.521498
166.316630	5240.725692	25.526515
166.278134	5254.277768	25.531533
166.930173	5261.735405	25.536551
167.122218	5271.217683	25.541568
166.905456	5276.638332	25.546586
167.199061	5293.374016	25.551603
167.373082	5297.940029	25.556621
167.899276	5306.388828	25.561639
167.940940	5327.709848	25.566656
168.091640	5329.482218	25.571674
168.389393	5329.725949	25.576691
168.329818	5331.980479	25.581709
168.606120	5336.168855	25.586727
168.764528	5349.715195	25.591744
168.557425	5351.506633	25.596762
168.774522	5362.120523	25.601779
169.123226	5371.636784	25.606797
169.560904	5384.824248	25.611815
169.714051	5391.347757	25.616832
170.011418	5397.763910	25.621850
170.346371	5402.912120	25.626867
170.239177	5395.791173	25.631885
170.805580	5398.850965	25.636903
170.827407	5390.083072	25.641920
170.921137	5389.474540	25.646938
171.001542	5406.819794	25.651955
171.198471	5412.579188	25.656973
171.275993	5413.235849	25.661991
171.411266	5414.775292	25.667008
171.602188	5421.499698	25.672026
171.675449	5424.304831	25.677044
171.901917	5443.382278	25.682061
171.951702	5438.042065	25.687079
171.982024	5440.016310	25.692096
172.476607	5454.742822	25.697114
172.481184	5467.644486	25.702132
172.613896	5465.247957	25.707149
172.751118	5477.238476	25.712167
172.718842	5489.500430	25.717184
173.190156	5487.635390	25.722202
173.260038	5496.357520	25.727220
173.215464	5526.456677	25.732237
173.664713	5526.116926	25.737255
173.462985	5530.922420	25.742272
174.030806	5551.314697	25.747290
174.043101	5547.896096	25.752308
173.871026	5561.857261	25.757325
174.384781	5576.263311	25.762343
174.762521	5584.561202	25.767360
174.829241	5575.101349	25.772378
174.699241	5588.171097	25.777396
175.079888	5611.050966	25.782413
175.431817	5604.533619	25.787431
175.562746	5619.998614	25.792448
175.832722	5632.833637	25.797466
176.210212	5636.568222	25.802484
176.355852	5646.817659	25.807501
176.189953	5633.069972	25.812519
175.953112	5647.517647	25.817536
176.529331	5660.623337	25.822554
176.888724	5656.840086	25.827572
176.780887	5664.407172	25.832589
177.112945	5681.939474	25.837607
177.442543	5685.969477	25.842624
177.751515	5689.820957	25.847642
177.969407	5692.229657	25.852660
178.011119	5697.050822	25.857677
178.370735	5702.028863	25.862695
178.196825	5718.284769	25.867712
178.224204	5721.209391	25.872730
178.292555	5727.150859	25.877748
178.360276	5746.012369	25.882765
178.679061	5759.408856	25.887783
179.191421	5768.451691	25.892800
179.245214	5780.016764	25.897818
179.715309	5783.057922	25.902836
179.579683	5795.074160	25.907853
179.841652	5791.331422	25.912871
179.723972	5815.404616	25.917888
179.948211	5811.551552	25.922906
180.566279	5824.292876	25.927924
180.617629	5836.050572	25.932941
180.786700	5832.342893	25.937959
180.797676	5848.633698	25.942976
181.146927	5861.508554	25.947994
181.196216	5870.805321	25.953012
181.044857	5876.342152	25.958029
181.551849	5882.042513	25.963047
181.776975	5885.145510	25.968064
181.894114	5901.090358	25.973082
182.120349	5921.819268	25.978100
181.882840	5921.629430	25.983117
182.279668	5937.729644	25.988135
183.064557	5941.040857	25.993152
183.029006	5956.189551	25.998170
183.261837	5958.789574	26.003188
183.077683	5973.647050	26.008205
183.412425	5975.485116	26.013223
183.932502	5977.804454	26.018240
183.809331	5980.038887	26.023258
184.016901	5993.790299	26.028276
184.362629	6010.098315	26.033293
184.648152	6001.313997	26.038311
184.759536	6015.450745	26.043328
184.782552	6033.285063	26.048346
185.083387	6033.212461	26.053364
185.058510	6043.354912	26.058381
185.295398	6050.183820	26.063399
185.487049	6064.125384	26.068416
185.684211	6070.515869	26.073434
185.790744	6066.955535	26.078452
185.985439	6084.742587	26.083469
186.128142	6095.464590	26.088487
186.449252	6094.353690	26.093504
186.420587	6107.204670	26.098522
186.675034	6120.139539	26.103540
186.890238	6134.776679	26.108557
187.008693	6132.938476	26.113575
187.211915	6147.860370	26.118592
187.331107	6166.764269	26.123610
187.770949	6149.143108	26.128628
187.816101	6167.263759	26.133645
187.954131	6183.474015	26.138663
188.128853	6180.629352	26.143680
188.204772	6192.183187	26.148698
188.638239	6206.562150	26.153716
188.391128	6214.047011	26.158733
188.567189	6224.490270	26.163751
189.339018	6232.797304	26.168768
189.485188	6246.408662	26.173786
189.809911	6238.236805	26.178804
189.804419	6250.121576	26.183821
190.151829	6269.165036	26.188839
190.084396	6262.093038	26.193856
190.456564	6271.229471	26.198874
190.906456	6270.624169	26.203892
190.958213	6292.781290	26.208909
190.835972	6291.045137	26.213927
191.057423	6291.438568	26.218944
190.891048	6298.493444	26.223962
191.739375	6312.812491	26.228980
191.745235	6328.400488	26.233997
191.700619	6328.560716	26.239015
191.927870	6333.092227	26.244032
191.584924	6338.820037	26.249050
192.568902	6358.071705	26.254068
192.393659	6371.221262	26.259085
192.712122	6376.372524	26.264103
192.983958	6385.315333	26.269120
193.067362	6408.028176	26.274138
193.481447	6403.448055	26.279156
193.501185	6425.453133	26.284173
193.923261	6425.999239	26.289191
193.887295	6432.996354	26.294208
193.960365	6457.487114	26.299226
194.252933	6463.741456	26.304244
194.552637	6469.238479	26.309261
194.518539	6484.415005	26.314279
194.772740	6491.839850	26.319296
195.008991	6501.888170	26.324314
195.466846	6509.501426	26.329332
195.402259	6521.730146	26.334349
195.784595	6521.541658	26.339367
196.340282	6530.917238	26.344384
196.010471	6552.472324	26.349402
196.306344	6548.938038	26.354420
196.461240	6555.241986	26.359437
196.884632	6582.527025	26.364455
197.022237	6573.225764	26.369472
196.844511	6580.874956	26.374490
197.125673	6595.483488	26.379508
197.141891	6600.005115	26.384525
197.535416	6626.910801	26.389543
197.986975	6632.266958	26.394560
198.409510	6631.496040	26.399578
198.462807	6642.866488	26.404596
198.746415	6658.240273	26.409613
198.483228	6666.922879	26.414631
199.135553	6664.407072	26.419648
199.125147	6682.461107	26.424666
199.250340	6681.277843	26.429684
199.483760	6694.668778	26.434701
199.457814	6705.950781	26.439719
199.584798	6727.424184	26.444736
200.063724	6724.513313	26.449754
200.235338	6736.129682	26.454772
200.295590	6758.505016	26.459789
200.346636	6766.744979	26.464807
200.950754	6760.847050	26.469824
200.804237	6793.328468	26.474842
201.365173	6791.108178	26.479860
201.001954	6794.651384	26.484877
201.398984	6805.729536	26.489895
201.701506	6813.676630	26.494912
201.967126	6831.421273	26.499930
202.135904	6844.307116	26.504948
202.211759	6842.245099	26.509965
202.140222	6862.285706	26.514983
202.606422	6857.924465	26.520000
202.910055	6878.553597	26.525018
203.278366	6899.960503	26.530036
203.506903	6907.993145	26.535053
203.656538	6904.726379	26.540071
203.855908	6916.420990	26.545088
204.054066	6925.963903	26.550106
204.387282	6922.040547	26.555124
204.344088	6925.944330	26.560141
204.479636	6948.171987	26.565159
204.994470	6946.886396	26.570176
205.251384	6967.617898	26.575194
205.047485	6982.038488	26.580212
205.336843	6986.485078	26.585229
205.218799	7001.831953	26.590247
205.858641	7008.055804	26.595264
205.982185	7034.431087	26.600282
206.405527	7038.692464	26.605300
206.613314	7044.021376	26.610317
206.653703	7056.602548	26.615335
207.451967	7069.984579	26.620352
207.186573	7077.361807	26.625370
207.409734	7083.654666	26.630388
207.769727	7095.181039	26.635405
207.752363	7109.256583	26.640423
208.282598	7100.768278	26.645440
208.213012	7121.840744	26.650458
208.446058	7129.115794	26.655476
208.582795	7140.930427	26.660493
208.825526	7154.276099	26.665511
209.041356	7161.787167	26.670528
209.229477	7170.110197	26.675546
209.542698	7180.859058	26.680564
209.503351	7196.964232	26.685581
209.420821	7201.742619	26.690599
209.899710	7212.814596	26.695616
210.002255	7233.191549	26.700634
210.396835	7239.715241	26.705652
210.727216	7254.788057	26.710669
210.744374	7268.420074	26.715687
211.228059	7267.762674	26.720704
210.980277	7276.851081	26.725722
211.434689	7288.950366	26.730740
212.152748	7303.406884	26.735757
212.093258	7314.606651	26.740775
212.353517	7303.955831	26.745792
212.312492	7319.732155	26.750810
212.596106	7342.793645	26.755828
212.935628	7340.033348	26.760845
212.868410	7357.195650	26.765863
213.165264	7362.114507	26.770880
213.230550	7377.987504	26.775898
213.353542	7400.900013	26.780916
213.907718	7387.442777	26.785933
213.446626	7402.316708	26.790951
214.145125	7411.794418	26.795968
214.392828	7422.727581	26.800986
214.676137	7441.789364	26.806004
214.966199	7452.375252	26.811021
215.147690	7458.148191	26.816039
215.397392	7457.915487	26.821056
215.612405	7475.773205	26.826074
215.648018	7480.912575	26.831092
215.837854	7489.363096	26.836109
215.926906	7507.528421	26.841127
216.250647	7511.454315	26.846144
216.465936	7525.224684	26.851162
216.385710	7542.783975	26.856180
216.927448	7547.389021	26.861197
216.827438	7569.231971	26.866215
217.082815	7573.969499	26.871232
217.071620	7601.358165	26.876250
217.417937	7612.573673	26.881268
217.942715	7629.315313	26.886285
218.387697	7645.358884	26.891303
218.750048	7646.486799	26.896320
219.222521	7658.065068	26.901338
218.961284	7663.265452	26.906356
219.485645	7671.870223	26.911373
219.715778	7698.903239	26.916391
220.112413	7694.370542	26.921408
219.805947	7688.624588	26.926426
219.939338	7703.449228	26.931444
220.552142	7714.819198	26.936461
220.843064	7733.055342	26.941479
221.182571	7723.640429	26.946496
221.205957	7741.244229	26.951514
221.011686	7752.698200	26.956532
221.571653	7754.603176	26.961549
221.546890	7785.473714	26.966567
221.658533	7771.969679	26.971584
222.103553	7786.215045	26.976602
222.306605	7804.016033	26.981620
222.227122	7815.978815	26.986637
222.141706	7842.516061	26.991655
222.405100	7848.364596	26.996672
222.801055	7867.853301	27.001690
222.888104	7887.305729	27.006708
223.281072	7890.094613	27.011725
223.236585	7923.082122	27.016743
223.304360	7930.723617	27.021760
224.304607	7956.576410	27.026778
224.408064	7970.160083	27.031796
224.880518	7988.015934	27.036813
224.890559	7997.113272	27.041831
225.068432	7998.489950	27.046848
225.850904	8015.824244	27.051866
225.640699	8021.729184	27.056884
226.388249	8035.166118	27.061901
226.563046	8053.973259	27.066919
226.484780	8049.404855	27.071936
227.078729	8048.206916	27.076954
226.982508	8071.162190	27.081972
227.863853	8074.998285	27.086989
227.556136	8086.445279	27.092007
227.655373	8078.179049	27.097024
227.978903	8090.279345	27.102042
228.100265	8100.198029	27.107060
228.357496	8105.505724	27.112077
228.336725	8123.624550	27.117095
228.549698	8133.268141	27.122112
228.933658	8141.747530	27.127130
228.910583	8151.387668	27.132148
229.381313	8165.172237	27.137165
229.355384	8177.220951	27.142183
229.697346	8186.136628	27.147200
229.932273	8196.034999	27.152218
229.681212	8210.689006	27.157236
230.181525	8214.445631	27.162253
230.283621	8237.759031	27.167271
230.488398	8245.462286	27.172288
230.989834	8257.096855	27.177306
230.796490	8281.813338	27.182324
231.334810	8296.456491	27.187341
231.374960	8305.580530	27.192359
231.306095	8320.121766	27.197376
232.133594	8341.736615	27.202394
232.156305	8354.780989	27.207412
232.254938	8362.276578	27.212429
232.584033	8391.654452	27.217447
232.849239	8397.176765	27.222464
233.158723	8413.178159	27.227482
233.029221	8440.910034	27.232500
233.714712	8453.624997	27.237517
233.543184	8470.658453	27.242535
233.849753	8482.937521	27.247552
234.174753	8501.926714	27.252570
234.180888	8521.892739	27.257588
234.683259	8531.649367	27.262605
235.412489	8551.839192	27.267623
235.427785	8575.479400	27.272640
235.891679	8575.391623	27.277658
236.185120	8591.290293	27.282676
236.412476	8604.693295	27.287693
236.886578	8601.111730	27.292711
237.168246	8622.402957	27.297728
237.572763	8630.887870	27.302746
237.508167	8628.903228	27.307764
237.454931	8629.336680	27.312781
237.709672	8645.938970	27.317799
238.198887	8652.024560	27.322816
238.376155	8662.160425	27.327834
238.379997	8692.462372	27.332852
238.829611	8693.593252	27.337869
238.865137	8699.991074	27.342887
238.749695	8714.713684	27.347904
238.966422	8728.585689	27.352922
239.077871	8750.664661	27.357940
239.600701	8763.602163	27.362957
239.959452	8783.503056	27.367975
239.967067	8794.044424	27.372992
240.357991	8809.727872	27.378010
240.928578	8820.061055	27.383028
241.073304	8836.732172	27.388045
241.220569	8844.448388	27.393063
241.378091	8860.885809	27.398080
241.847481	8863.666945	27.403098
241.800122	8874.984748	27.408116
242.436406	8900.223426	27.413133
242.418492	8899.009335	27.418151
242.574819	8920.769158	27.423168
242.912266	8930.981088	27.428186
243.234390	8947.652891	27.433204
243.758987	8966.231470	27.438221
244.090251	8959.479858	27.443239
243.917044	8974.573066	27.448256
244.426836	8983.346396	27.453274
244.464719	8997.187581	27.458292
244.626557	9015.389051	27.463309
245.040017	9026.313998	27.468327
245.001923	9027.902977	27.473344
245.496508	9050.783916	27.478362
245.525496	9053.363052	27.483380
245.596684	9058.082673	27.488397
245.993539	9077.730265	27.493415
245.869486	9086.499859	27.498432
246.497920	9109.290977	27.503450
246.356867	9126.737605	27.508468
246.694115	9138.221173	27.513485
247.208546	9153.066802	27.518503
247.142523	9178.296916	27.523520
247.536535	9178.475947	27.528538
247.546869	9204.370952	27.533556
247.885341	9200.116886	27.538573
248.186271	9227.525994	27.543591
248.486391	9245.310158	27.548608
248.828668	9262.747829	27.553626
248.594538	9280.119436	27.558644
248.727071	9302.187800	27.563661
249.002646	9320.292011	27.568679
249.311091	9343.182122	27.573696
250.245614	9357.925317	27.578714
250.719634	9378.949376	27.583732
251.023612	9399.993731	27.588749
251.198535	9401.731829	27.593767
251.540849	9416.248537	27.598784
251.862737	9432.983908	27.603802
251.935363	9436.008075	27.608820
252.368516	9446.651960	27.613837
252.635178	9452.571447	27.618855
252.717394	9464.848231	27.623872
253.375515	9467.600599	27.628890
253.291756	9486.819334	27.633908
253.567395	9487.919201	27.638925
253.837168	9496.150365	27.643943
253.725469	9516.679924	27.648960
254.152750	9517.074825	27.653978
254.229101	9541.590257	27.658996
254.218552	9550.764363	27.664013
254.743368	9566.672185	27.669031
255.049375	9581.939522	27.674048
255.374217	9596.923300	27.679066
255.458378	9615.514090	27.684084
255.441540	9628.469935	27.689101
255.772748	9639.236389	27.694119
256.162630	9673.318395	27.699136
256.329722	9677.671751	27.704154
256.927320	9696.007481	27.709172
257.036514	9703.646118	27.714189
257.722800	9730.791409	27.719207
257.456384	9733.692134	27.724224
257.960766	9746.256917	27.729242
257.950192	9770.471964	27.734260
258.648483	9784.542481	27.739277
259.126777	9786.677094	27.744295
259.086519	9801.756948	27.749312
259.498001	9807.113734	27.754330
259.701834	9814.227046	27.759348
259.941515	9832.153430	27.764365
260.012534	9845.599107	27.769383
260.270226	9855.710599	27.774400
260.756630	9872.381383	27.779418
260.664180	9888.321583	27.784436
260.734446	9898.917119	27.789453
261.095726	9911.546686	27.794471
261.259458	9935.045366	27.799488
261.690484	9945.278696	27.804506
261.822326	9977.669289	27.809524
262.005984	9995.243520	27.814541
262.411265	10002.185702	27.819559
262.541354	10016.002260	27.824576
262.773257	10037.578555	27.829594
263.322969	10053.001382	27.834612
263.561284	10051.135805	27.839629
263.733177	10071.213400	27.844647
263.687774	10089.296767	27.849664
264.210909	10109.235125	27.854682
264.328811	10119.650387	27.859700
264.681900	10132.249971	27.864717
264.933875	10144.331368	27.869735
265.672664	10179.294996	27.874752
265.808616	10182.158347	27.879770
265.742596	10192.369328	27.884788
266.023397	10199.088761	27.889805
266.536844	10213.442359	27.894823
266.661692	10236.323955	27.899840
266.911244	10241.703752	27.904858
267.197213	10252.407990	27.909876
267.145420	10272.511832	27.914893
267.688438	10295.863172	27.919911
267.805880	10317.354795	27.924928
268.314058	10318.309873	27.929946
268.493144	10349.368256	27.934964
268.560937	10359.725790	27.939981
269.180350	10377.162132	27.944999
269.514068	10402.206670	27.950016
269.580740	10412.188624	27.955034
269.901625	10421.080680	27.960052
269.992586	10445.183818	27.965069
270.679630	10450.352610	27.970087
270.981255	10486.512729	27.975104
270.829579	10491.931449	27.980122
271.489165	10510.292517	27.985140
271.426927	10525.944722	27.990157
271.647639	10547.895417	27.995175
271.833751	10560.011663	28.000192
272.199745	10576.390336	28.005210
272.503365	10602.829141	28.010228
272.835410	10627.066760	28.015245
273.373698	10638.299106	28.020263
273.683415	10648.318187	28.025280
273.877746	10671.133749	28.030298
274.359752	10691.018185	28.035316
274.362097	10695.500721	28.040333
274.860689	10702.549880	28.045351
275.204706	10716.797251	28.050368
275.251261	10739.542828	28.055386
275.817553	10735.813971	28.060404
275.822708	10765.732768	28.065421
275.999632	10776.771335	28.070439
276.309742	10790.193982	28.075456
276.480293	10796.522229	28.080474
276.879106	10821.620461	28.085492
276.831481	10837.959138	28.090509
277.398473	10854.569545	28.095527
277.242701	10869.856240	28.100544
277.787719	10894.539606	28.105562
278.240977	10905.477371	28.110580
278.346714	10925.879764	28.115597
278.979956	10931.041075	28.120615
279.247716	10956.914407	28.125632
279.266780	10968.633164	28.130650
279.724482	10983.062071	28.135668
279.718611	10999.034732	28.140685
280.417955	11016.918655	28.145703
280.774680	11030.768691	28.150720
280.790565	11038.203591	28.155738
281.210410	11057.154900	28.160756
281.318001	11068.843319	28.165773
281.905643	11090.589049	28.170791
281.980674	11094.300156	28.175808
281.993436	11102.636929	28.180826
282.913160	11105.440835	28.185844
282.847047	11112.112499	28.190861
283.205612	11111.367740	28.195879
283.692014	11125.752632	28.200896
283.945680	11143.299195	28.205914
284.032380	11142.741251	28.210932
284.445492	11152.587533	28.215949
284.578846	11169.947616	28.220967
284.428568	11180.572620	28.225984
285.141076	11190.834217	28.231002
285.102039	11201.341550	28.236020
284.954357	11224.795958	28.241037
285.329330	11234.320846	28.246055
285.645557	11261.971980	28.251072
285.993568	11285.528794	28.256090
286.045333	11306.293571	28.261108
286.353670	11332.810005	28.266125
286.767444	11357.309378	28.271143
287.105039	11374.779269	28.276160
287.089815	11407.799019	28.281178
287.715431	11424.724922	28.286196
287.467089	11452.852743	28.291213
288.036662	11477.104325	28.296231
288.399327	11509.439300	28.301248
288.511134	11524.009461	28.306266
288.859443	11551.594324	28.311284
289.338052	11572.703224	28.316301
289.970113	11592.171564	28.321319
290.382053	11608.767445	28.326336
290.697539	11626.858980	28.331354
291.175592	11652.649769	28.336372
291.175637	11671.315155	28.341389
291.500391	11686.064525	28.346407
291.782117	11697.834881	28.351424
291.915567	11723.840403	28.356442
292.507850	11726.318853	28.361460
292.896202	11758.068601	28.366477
293.050244	11771.555716	28.371495
293.386221	11788.624491	28.376512
293.412025	11804.662040	28.381530
294.050161	11815.747892	28.386548
294.009574	11842.650684	28.391565
294.261667	11854.623038	28.396583
294.831309	11869.226461	28.401600
294.714651	11903.458480	28.406618
294.817433	11927.718665	28.411636
295.097459	11943.670149	28.416653
295.953601	11958.621765	28.421671
296.137019	11977.417886	28.426688
296.480102	12018.855968	28.431706
296.952923	12022.424231	28.436724
296.913557	12056.736754	28.441741
297.399148	12062.034758	28.446759
297.787513	12089.311347	28.451776
297.889427	12098.603018	28.456794
298.344959	12116.079403	28.461812
298.288840	12140.331538	28.466829
298.553016	12153.643157	28.471847
299.010598	12186.219060	28.476864
299.317495	12212.240779	28.481882
299.725296	12225.245032	28.486900
300.107564	12245.483551	28.491917
300.191084	12260.134697	28.496935
300.650890	12262.044213	28.501952
300.668329	12286.448280	28.506970
300.867991	12301.876049	28.511988
300.924414	12324.693131	28.517005
301.340038	12341.657906	28.522023
301.820073	12365.451305	28.527040
302.237299	12390.849916	28.532058
302.860554	12405.853102	28.537076
302.774697	12437.159479	28.542093
303.125524	12457.466501	28.547111
303.901947	12473.517571	28.552128
303.682590	12486.914225	28.557146
303.951243	12503.036761	28.562164
304.200751	12522.301642	28.567181
304.357349	12542.150818	28.572199
304.925197	12563.359704	28.577216
305.331215	12593.935704	28.582234
305.976512	12612.604107	28.587252
306.166633	12626.051292	28.592269
306.217252	12649.363044	28.597287
306.619174	12664.595364	28.602304
306.745450	12687.759122	28.607322
307.365062	12706.712395	28.612340
307.607809	12722.018392	28.617357
308.306729	12746.634989	28.622375
308.747180	12761.618334	28.627392
308.489217	12774.260450	28.632410
308.622335	12792.329890	28.637428
308.526684	12814.520402	28.642445
309.116658	12837.832979	28.647463
309.557284	12862.774593	28.652480
309.881335	12879.283888	28.657498
309.957041	12904.505017	28.662516
310.202058	12935.220197	28.667533
310.692912	12965.016954	28.672551
311.159544	12984.092004	28.677568
310.805267	13021.467127	28.682586
311.765401	13040.093369	28.687604
311.717618	13071.189789	28.692621
312.341374	13098.104468	28.697639
312.990146	13124.323213	28.702656
313.216798	13150.137507	28.707674
313.580110	13165.453909	28.712692
313.707979	13192.282194	28.717709
313.897053	13201.103044	28.722727
314.449890	13219.716533	28.727744
314.872125	13247.474852	28.732762
315.257065	13262.601804	28.737780
315.658401	13290.253339	28.742797
315.566944	13303.530206	28.747815
315.879626	13323.072403	28.752832
316.264744	13341.924971	28.757850
316.864992	13354.185943	28.762868
317.176989	13379.400216	28.767885
317.520653	13396.874434	28.772903
317.683185	13401.846545	28.777920
317.954069	13425.802192	28.782938
318.469122	13438.770756	28.787956
318.620927	13469.418843	28.792973
319.135042	13483.971453	28.797991
319.687051	13503.866674	28.803008
319.737274	13522.037322	28.808026
319.918305	13535.551378	28.813044
320.293468	13556.088990	28.818061
320.587192	13578.978869	28.823079
321.109104	13594.023571	28.828096
320.866606	13614.663486	28.833114
321.309612	13635.089106	28.838132
321.923710	13654.498285	28.843149
322.064508	13664.142165	28.848167
322.590650	13674.221862	28.853184
322.333317	13698.333103	28.858202
322.753260	13718.737428	28.863220
323.294217	13738.630037	28.868237
323.541373	13761.345064	28.873255
323.841305	13771.805830	28.878272
323.866065	13799.336163	28.883290
324.306275	13824.649681	28.888308
324.700460	13841.293337	28.893325
324.878621	13868.265705	28.898343
325.307183	13880.092143	28.903360
325.797339	13914.371362	28.908378
326.217102	13929.951792	28.913396
326.379672	13945.577957	28.918413
326.527286	13977.477474	28.923431
326.992122	13997.108770	28.928448
327.284303	14020.599989	28.933466
327.449119	14051.667813	28.938484
328.157399	14081.076018	28.943501
328.329440	14101.838635	28.948519
328.893712	14126.676613	28.953536
328.935082	14144.053517	28.958554
329.278678	14167.259054	28.963572
329.867352	14192.178199	28.968589
330.102989	14215.593951	28.973607
330.192235	14239.799924	28.978624
330.763272	14273.083054	28.983642
330.644589	14293.265187	28.988660
331.405334	14308.516885	28.993677
331.638979	14340.065594	28.998695
332.027171	14360.706081	29.003712
332.221511	14398.631846	29.008730
332.907801	14412.841578	29.013748
333.227395	14443.841975	29.018765
333.352786	14458.480284	29.023783
333.653439	14472.826394	29.028800
334.070135	14501.229223	29.033818
334.627174	14527.315682	29.038836
335.040984	14546.521086	29.043853
335.096060	14570.123260	29.048871
336.076464	14591.791346	29.053888
336.080217	14617.778816	29.058906
335.932914	14623.029536	29.063924
336.490968	14652.219340	29.068941
336.837970	14677.155581	29.073959
337.113333	14699.487403	29.078976
337.638681	14726.014426	29.083994
337.914203	14737.726544	29.089012
338.238536	14761.401060	29.094029
338.541923	14781.840189	29.099047
339.015596	14806.021199	29.104064
339.396990	14836.668519	29.109082
339.751304	14862.514823	29.114100
340.304766	14886.224098	29.119117
340.203623	14906.653105	29.124135
340.887494	14921.385376	29.129152
340.941453	14947.642454	29.134170
341.218474	14966.992353	29.139188
341.255751	14989.780070	29.144205
341.974029	15022.178215	29.149223
342.000298	15034.174521	29.154240
342.256967	15062.485022	29.159258
342.847887	15085.031508	29.164276
343.379857	15112.574664	29.169293
343.220161	15139.627106	29.174311
343.776914	15166.354541	29.179328
344.014323	15193.346076	29.184346
344.146217	15227.690489	29.189364
344.597018	15236.883648	29.194381
345.067718	15274.220348	29.199399
345.414242	15290.487212	29.204416
345.860484	15318.730528	29.209434
346.086138	15330.798077	29.214452
346.943871	15359.236576	29.219469
346.790424	15384.322918	29.224487
347.276809	15407.966817	29.229504
347.771989	15426.433176	29.234522
347.976128	15450.021399	29.239540
348.565472	15461.890149	29.244557
348.872737	15485.267486	29.249575
348.940574	15505.355611	29.254592
349.142316	15537.050601	29.259610
349.537858	15562.749326	29.264628
350.043540	15590.069089	29.269645
350.400983	15619.516057	29.274663
350.798504	15634.715628	29.279680
350.953490	15656.441353	29.284698
351.377227	15701.555812	29.289716
351.840662	15711.601442	29.294733
351.793709	15747.018399	29.299751
351.938377	15772.401177	29.304768
352.698095	15812.359764	29.309786
353.121850	15841.324870	29.314804
353.609197	15859.867094	29.319821
354.004471	15887.905459	29.324839
354.290749	15909.077029	29.329856
354.609000	15932.117450	29.334874
355.151415	15967.531910	29.339892
355.721949	15981.108039	29.344909
356.150207	16009.172676	29.349927
356.016869	16032.527561	29.354944
356.272031	16059.962072	29.359962
356.233767	16092.276324	29.364980
356.834027	16111.771100	29.369997
357.451328	16142.183204	29.375015
357.914217	16176.239954	29.380032
358.208725	16201.563915	29.385050
358.832822	16238.618912	29.390068
359.327693	16256.487283	29.395085
359.338199	16290.136808	29.400103
359.664928	16311.046848	29.405120
360.192635	16333.156279	29.410138
360.148178	16369.422178	29.415156
360.846983	16398.232402	29.420173
361.165159	16427.154537	29.425191
361.515798	16452.893607	29.430208
361.939984	16481.401074	29.435226
362.226401	16509.731205	29.440244
363.053302	16534.861956	29.445261
362.965064	16546.260414	29.450279
363.412745	16577.669224	29.455296
363.653087	16596.270496	29.460314
364.010235	16624.133574	29.465332
364.666453	16650.728738	29.470349
364.379126	16696.234717	29.475367
364.983995	16708.949843	29.480384
365.369999	16736.861929	29.485402
365.440583	16774.044412	29.490420
366.159277	16807.576205	29.495437
366.320984	16835.115741	29.500455
365.996657	16874.222261	29.505472
367.266532	16899.712162	29.510490
367.714084	16935.488032	29.515508
368.023484	16957.443696	29.520525
368.436351	16989.869464	29.525543
369.114945	16997.924070	29.530560
369.529717	17017.245696	29.535578
369.621689	17045.824880	29.540596
370.269657	17054.127336	29.545613
370.491770	17090.141042	29.550631
370.449862	17102.736524	29.555648
370.763808	17117.013384	29.560666
370.949863	17158.145224	29.565684
371.792448	17176.352705	29.570701
371.741631	17208.995934	29.575719
371.777481	17239.709636	29.580736
372.643709	17271.937971	29.585754
372.486418	17302.496169	29.590772
372.696010	17334.005718	29.595789
373.513604	17374.918503	29.600807
373.970398	17407.419788	29.605824
374.491865	17447.519496	29.610842
374.661275	17477.938825	29.615860
375.260655	17504.779648	29.620877
375.536876	17537.892749	29.625895
375.711104	17574.591691	29.630912
376.233884	17605.362627	29.635930
376.596422	17638.362332	29.640948
376.989901	17670.007604	29.645965
377.424896	17697.536445	29.650983
377.904500	17734.311311	29.656000
378.109311	17757.582706	29.661018
378.243041	17795.583049	29.666036
378.642192	17821.516418	29.671053
379.131291	17869.469776	29.676071
379.424598	17905.620071	29.681088
380.220537	17934.985978	29.686106
380.105128	17980.191143	29.691124
380.850909	18005.689095	29.696141
381.238625	18044.005816	29.701159
381.529801	18074.924723	29.706176
382.097553	18102.761735	29.711194
382.247947	18158.970928	29.716212
382.900527	18182.566071	29.721229
383.465411	18220.825502	29.726247
384.008846	18243.024739	29.731264
384.315391	18269.355628	29.736282
384.491834	18305.109953	29.741300
385.376122	18322.859360	29.746317
385.716710	18356.879348	29.751335
385.937156	18381.236772	29.756352
386.257098	18405.645552	29.761370
386.680666	18449.567843	29.766388
387.180580	18464.239149	29.771405
387.681152	18494.851456	29.776423
387.777227	18524.102491	29.781440
388.484724	18547.433678	29.786458
388.628290	18578.054773	29.791476
388.827320	18604.834360	29.796493
389.418381	18624.711975	29.801511
389.405111	18652.379641	29.806528
389.997277	18690.235212	29.811546
390.283544	18721.427284	29.816564
391.134724	18754.083485	29.821581
391.019333	18784.076234	29.826599
391.071002	18809.841635	29.831616
391.541920	18845.622478	29.836634
391.808200	18886.814673	29.841652
392.615731	18913.088893	29.846669
393.083948	18942.107234	29.851687
393.436924	18981.986284	29.856704
393.898112	19017.343449	29.861722
394.130702	19042.171202	29.866740
394.652824	19061.091196	29.871757
395.167763	19091.856718	29.876775
395.519176	19122.769175	29.881792
396.015543	19146.052587	29.886810
396.601821	19179.127095	29.891828
396.474194	19192.507680	29.896845
397.071509	19213.337181	29.901863
397.260077	19245.281058	29.906880
397.964778	19274.030667	29.911898
398.189528	19313.301116	29.916916
398.555983	19340.763613	29.921933
399.047677	19365.389735	29.926951
399.393366	19395.561095	29.931968
400.131161	19415.880450	29.936986
400.235365	19448.165020	29.942004
400.468397	19473.453690	29.947021
400.821208	19503.064390	29.952039
400.918890	19537.563686	29.957056
401.419430	19577.394508	29.962074
401.600680	19611.807605	29.967092
402.221376	19646.286785	29.972109
402.961485	19676.060721	29.977127
403.080671	19719.838074	29.982144
403.590822	19752.308298	29.987162
403.802709	19790.312853	29.992180
404.335879	19831.844735	29.997197
405.006910	19865.483602	30.002215
404.937025	19909.753101	30.007232
405.871767	19929.512333	30.012250
405.988187	19965.822484	30.017268
406.606959	19998.289399	30.022285
407.011551	20027.112041	30.027303
406.905033	20061.220523	30.032320
408.014413	20095.829443	30.037338
408.761648	20124.113107	30.042356
409.282671	20147.168379	30.047373
409.610670	20175.259792	30.052391
409.745925	20210.515754	30.057408
410.353057	20242.108470	30.062426
410.392893	20275.589321	30.067444
410.976292	20296.012554	30.072461
411.430542	20320.072387	30.077479
411.682872	20354.812640	30.082496
412.184159	20391.009565	30.087514
412.322171	20425.447250	30.092532
412.942308	20461.635695	30.097549
413.270583	20496.031001	30.102567
413.460442	20530.684204	30.107584
413.933222	20558.793290	30.112602
414.302987	20592.959621	30.117620
414.507328	20628.520355	30.122637
415.584830	20669.327260	30.127655
415.586991	20704.612589	30.132672
416.273226	20744.207330	30.137690
416.404985	20777.420123	30.142708
416.543666	20812.769802	30.147725
417.218255	20847.007606	30.152743
417.252044	20889.015758	30.157760
418.290078	20923.184112	30.162778
418.837599	20958.545273	30.167796
419.153813	20993.497007	30.172813
419.848477	21021.942246	30.177831
419.535352	21060.865891	30.182848
420.200430	21096.751847	30.187866
421.053608	21122.627812	30.192884
421.235747	21164.199003	30.197901
421.714642	21178.764228	30.202919
421.833603	21215.078227	30.207936
422.316858	21239.178722	30.212954
423.137607	21263.873007	30.217972
422.919353	21301.572166	30.222989
423.549797	21336.906207	30.228007
423.362493	21378.360893	30.233024
424.090595	21405.544599	30.238042
424.497044	21447.281187	30.243060
424.840200	21476.742440	30.248077
425.439701	21525.577264	30.253095
425.596068	21566.098870	30.258112
426.068542	21600.160369	30.263130
426.700375	21639.802483	30.268148
426.898629	21682.693596	30.273165
427.335684	21708.748121	30.278183
427.972866	21758.028332	30.283200
428.311652	21789.170103	30.288218
428.740904	21821.459036	30.293236
429.040834	21874.086105	30.298253
429.434327	21905.911239	30.303271
429.823262	21954.231852	30.308288
430.587842	21992.821613	30.313306
431.015244	22044.702798	30.318324
431.436501	22078.731163	30.323341
431.871389	22119.592738	30.328359
432.153865	22166.875123	30.333376
432.574666	22202.557873	30.338394
433.094082	22241.109931	30.343412
433.787675	22289.645987	30.348429
434.139722	22322.606181	30.353447
434.489228	22366.927816	30.358464
434.969895	22400.920191	30.363482
435.332396	22438.498961	30.368500
435.579739	22485.810124	30.373517
436.429932	22512.336793	30.378535
436.889490	22572.410633	30.383552
436.958414	22599.705344	30.388570
437.872876	22638.807899	30.393588
438.116588	22688.431876	30.398605
438.878602	22712.914091	30.403623
439.378950	22762.330246	30.408640
439.897153	22797.160820	30.413658
440.470561	22824.574246	30.418676
440.402837	22867.953889	30.423693
440.994880	22896.539111	30.428711
441.652223	22935.812626	30.433728
442.130731	22960.006241	30.438746
442.716075	22995.715466	30.443764
442.684485	23036.120304	30.448781
443.063128	23059.657260	30.453799
443.576114	23104.486750	30.458816
443.842421	23148.176090	30.463834
444.432849	23189.296763	30.468852
444.737219	23231.407856	30.473869
445.277404	23274.348902	30.478887
445.721242	23310.657774	30.483904
446.019700	23356.138420	30.488922
446.825209	23384.130912	30.493940
447.096802	23436.120973	30.498957
447.770406	23457.026681	30.503975
447.894602	23501.744940	30.508992
448.407469	23537.831566	30.514010
449.209317	23573.627600	30.519028
449.461502	23616.514667	30.524045
450.202018	23641.050666	30.529063
450.072768	23673.769851	30.534080
450.868568	23721.299612	30.539098
451.331375	23744.233812	30.544116
451.385583	23786.966411	30.549133
452.568457	23821.756901	30.554151
452.462095	23850.799920	30.559168
453.025683	23882.933347	30.564186
453.461961	23923.218704	30.569204
453.182478	23957.585985	30.574221
453.910972	23992.212316	30.579239
454.290873	24034.658247	30.584256
454.891809	24075.897593	30.589274
455.406237	24113.808161	30.594292
455.580749	24152.140921	30.599309
456.399982	24189.458737	30.604327
456.602548	24233.230788	30.609344
456.895959	24279.517414	30.614362
457.528316	24319.351778	30.619380
457.781276	24368.278922	30.624397
458.608545	24407.822610	30.629415
458.905480	24452.771822	30.634432
459.114212	24507.664622	30.639450
459.588722	24540.233511	30.644468
460.107987	24594.012292	30.649485
460.524106	24644.256846	30.654503
461.153360	24694.728066	30.659520
461.319423	24736.602389	30.664538
461.909354	24780.172957	30.669556
461.961797	24838.533776	30.674573
463.041921	24881.127724	30.679591
463.461714	24939.882289	30.684608
463.811995	24982.332315	30.689626
464.547645	25028.405847	30.694644
464.819253	25083.778973	30.699661
465.535932	25126.638692	30.704679
466.139543	25164.849088	30.709696
466.415106	25221.906320	30.714714
467.236859	25259.326985	30.719732
467.413971	25298.535580	30.724749
467.750053	25346.691601	30.729767
468.364603	25377.611349	30.734784
468.721490	25431.807589	30.739802
469.203219	25470.584510	30.744820
469.774780	25526.369940	30.749837
470.249707	25571.781529	30.754855
470.937488	25608.436569	30.759872
471.215592	25662.296452	30.764890
472.028207	25705.289989	30.769908
472.347103	25756.004939	30.774925
473.150419	25792.158652	30.779943
473.684015	25840.437930	30.784960
473.802080	25874.342658	30.789978
474.235752	25905.400533	30.794996
474.413628	25950.496377	30.800013
474.796850	25994.063222	30.805031
475.361815	26048.526629	30.810048
475.972059	26100.560197	30.815066
476.627176	26132.559677	30.820084
476.812758	26182.449427	30.825101
477.296499	26228.444839	30.830119
477.996056	26279.110954	30.835136
478.208919	26330.983860	30.840154
479.119952	26375.640907	30.845172
479.011687	26423.529636	30.850189
479.573619	26461.992697	30.855207
479.974818	26516.222863	30.860224
480.346336	26562.199881	30.865242
481.381815	26608.051382	30.870260
481.823489	26660.903136	30.875277
482.284072	26703.329686	30.880295
483.203608	26742.970735	30.885312
483.384046	26785.642573	30.890330
483.852968	26820.715024	30.895348
484.042482	26865.779785	30.900365
484.472773	26900.565426	30.905383
485.110243	26938.575423	30.910400
485.495086	26990.756222	30.915418
486.171013	27022.454233	30.920436
486.576112	27072.720308	30.925453
486.778442	27120.751992	30.930471
487.179724	27160.019197	30.935488
487.653503	27200.697183	30.940506
488.033980	27244.797592	30.945524
488.587706	27292.705361	30.950541
489.439690	27336.447229	30.955559
489.580572	27391.748438	30.960576
489.619382	27439.937399	30.965594
490.675175	27489.150641	30.970612
491.071907	27544.599275	30.975629
491.605187	27599.684795	30.980647
492.435790	27647.393154	30.985664
492.360116	27689.371415	30.990682
493.257474	27741.923930	30.995700
493.471596	27795.441408	31.000717
494.263800	27840.920022	31.005735
495.260012	27881.664580	31.010752
495.232771	27938.657843	31.015770
495.718409	27972.755071	31.020788
496.181135	28026.383547	31.025805
496.532095	28074.475293	31.030823
497.373771	28123.668981	31.035840
497.803060	28183.688561	31.040858
498.218087	28230.148622	31.045876
498.809560	28275.910811	31.050893
499.400805	28331.295064	31.055911
500.025257	28368.499584	31.060928
500.308880	28424.793123	31.065946
500.886141	28467.163665	31.070964
501.766376	28516.957797	31.075981
501.938842	28565.029956	31.080999
502.555955	28613.369388	31.086016
502.801285	28665.824369	31.091034
503.451866	28717.654054	31.096052
503.738142	28761.464724	31.101069
504.128522	28810.763422	31.106087
505.185643	28867.062899	31.111104
505.464467	28918.494090	31.116122
505.820577	28959.454354	31.121140
506.420138	29019.704176	31.126157
506.975368	29068.951086	31.131175
507.600816	29116.842543	31.136192
507.840096	29165.047265	31.141210
508.445136	29196.865086	31.146228
508.853941	29258.551216	31.151245
509.275624	29320.232277	31.156263
510.381446	29357.151033	31.161280
510.493764	29408.923552	31.166298
511.012630	29469.645739	31.171316
511.570746	29511.987280	31.176333
511.839847	29568.255351	31.181351
512.957265	29607.295997	31.186368
513.284851	29663.684051	31.191386
514.039635	29705.898870	31.196404
514.501764	29748.846846	31.201421
514.713133	29804.664602	31.206439
515.500882	29842.507791	31.211456
515.725334	29893.534381	31.216474
516.096203	29931.673902	31.221492
516.868182	29988.304969	31.226509
516.876256	30040.235418	31.231527
518.010382	30074.317789	31.236544
517.804838	30124.722090	31.241562
518.853758	30166.567535	31.246580
519.172487	30215.771615	31.251597
519.267347	30256.276482	31.256615
520.158012	30302.575002	31.261632
520.437836	30347.577013	31.266650
520.815631	30397.305037	31.271668
521.703946	30441.420986	31.276685
521.747789	30501.351376	31.281703
522.382544	30549.620667	31.286720
522.783787	30614.190282	31.291738
523.366311	30667.258032	31.296756
523.912883	30719.644067	31.301773
524.153187	30778.968655	31.306791
525.009581	30826.712982	31.311808
525.440565	30890.518292	31.316826
525.900317	30954.546247	31.321844
526.888126	30998.091816	31.326861
527.671403	31052.714578	31.331879
528.541711	31101.788849	31.336896
528.707429	31155.659046	31.341914
529.155895	31193.791618	31.346932
529.936780	31248.538436	31.351949
529.810660	31301.539189	31.356967
530.958600	31355.443102	31.361984
531.464360	31407.828468	31.367002
531.781082	31456.755523	31.372020
532.356518	31506.864160	31.377037
532.701800	31563.208035	31.382055
533.205276	31614.745616	31.387072
534.027244	31673.790802	31.392090
534.505698	31732.867781	31.397108
535.058596	31791.557154	31.402125
535.281849	31841.889090	31.407143
535.806875	31894.045523	31.412160
536.391293	31961.748272	31.417178
536.872376	32015.414292	31.422196
537.195102	32069.172938	31.427213
537.715322	32121.106802	31.432231
538.532338	32190.409593	31.437248
538.795089	32243.585474	31.442266
539.612207	32307.145833	31.447284
540.302808	32370.528560	31.452301
540.871498	32439.381163	31.457319
541.232647	32493.939380	31.462336
541.594266	32550.185869	31.467354
542.232912	32616.989145	31.472372
542.977448	32675.741244	31.477389
543.409949	32731.411743	31.482407
543.846140	32786.289770	31.487424
544.322370	32855.979720	31.492442
544.940249	32904.693694	31.497460
545.916285	32964.178396	31.502477
546.357687	33037.396415	31.507495
547.224239	33083.684128	31.512512
547.526941	33151.346511	31.517530
547.853389	33205.259445	31.522548
548.872937	33245.536102	31.527565
549.185442	33303.307786	31.532583
549.854341	33349.745652	31.537600
550.143351	33408.259978	31.542618
550.990718	33465.097979	31.547636
551.966904	33511.778901	31.552653
551.917372	33567.370829	31.557671
552.717125	33620.408324	31.562688
553.155234	33674.181128	31.567706
553.684911	33711.867035	31.572724
554.383030	33751.002016	31.577741
554.861591	33811.452296	31.582759
555.228510	33846.767084	31.587776
555.569157	33902.377544	31.592794
556.577066	33950.130466	31.597812
557.131178	33987.112340	31.602829
557.563218	34047.700501	31.607847
558.103834	34084.508089	31.612864
558.848148	34140.033565	31.617882
559.094830	34192.025038	31.622900
559.757544	34247.097294	31.627917
559.901745	34312.679082	31.632935
560.422037	34352.946175	31.637952
561.029533	34408.214255	31.642970
561.497955	34474.784409	31.647988
562.022443	34531.250034	31.653005
562.776625	34594.721667	31.658023
563.443264	34647.071014	31.663040
563.788015	34701.291546	31.668058
564.308898	34766.910502	31.673076
565.369845	34816.105506	31.678093
565.628977	34880.916100	31.683111
566.237092	34940.553470	31.688128
566.730228	34991.133665	31.693146
567.030448	35053.823623	31.698164
568.163671	35121.160371	31.703181
568.404595	35176.781814	31.708199
569.156339	35243.834985	31.713216
569.839881	35298.761851	31.718234
570.493978	35359.604894	31.723252
571.103880	35410.807613	31.728269
571.173678	35472.391531	31.733287
571.628926	35534.502059	31.738304
572.027815	35595.164047	31.743322
572.905631	35668.740362	31.748340
573.458621	35723.503918	31.753357
574.238128	35804.185514	31.758375
574.796536	35866.100222	31.763392
575.589208	35915.330001	31.768410
576.151311	35978.052436	31.773428
576.817747	36031.115965	31.778445
577.680582	36095.603805	31.783463
578.165436	36137.035893	31.788480
578.972093	36192.131324	31.793498
579.373327	36260.306725	31.798516
580.381516	36304.985488	31.803533
580.521124	36364.926019	31.808551
581.172403	36417.311462	31.813568
581.925771	36472.082012	31.818586
581.996452	36527.221327	31.823604
582.798493	36572.865933	31.828621
583.412256	36646.442580	31.833639
583.651462	36699.588225	31.838656
584.254581	36751.231427	31.843674
584.632187	36831.397047	31.848692
585.509713	36881.208793	31.853709
585.802355	36943.284784	31.858727
586.403943	37018.212673	31.863744
586.968468	37071.886338	31.868762
587.710941	37143.366880	31.873780
588.440213	37198.386647	31.878797
588.753924	37258.938898	31.883815
589.331527	37326.401055	31.888832
590.115502	37390.038568	31.893850
590.450114	37456.676577	31.898868
591.311432	37523.098278	31.903885
591.792837	37584.217261	31.908903
592.169537	37643.071716	31.913920
592.882793	37681.603563	31.918938
593.495376	37756.870412	31.923956
594.329126	37810.223955	31.928973
594.493236	37878.488855	31.933991
594.878728	37926.913990	31.939008
595.383762	37981.199904	31.944026
595.909193	38055.608074	31.949044
596.778082	38114.123793	31.954061
597.459329	38187.269392	31.959079
597.787842	38256.935231	31.964096
598.438442	38317.659375	31.969114
598.894316	38385.824242	31.974132
600.219734	38446.708630	31.979149
600.189758	38520.651883	31.984167
600.809318	38588.111771	31.989184
601.343775	38645.835418	31.994202
601.998240	38711.762220	31.999220
602.774149	38792.198854	32.004237
603.182192	38855.594339	32.009255
604.268850	38931.014872	32.014272
604.829768	38993.293360	32.019290
605.682819	39060.204991	32.024308
606.282720	39122.932024	32.029325
607.255498	39194.010024	32.034343
607.537757	39240.372337	32.039360
608.481464	39297.121217	32.044378
608.659780	39367.725251	32.049396
609.637977	39422.776840	32.054413
610.340349	39476.797797	32.059431
610.631072	39547.778513	32.064448
611.354637	39595.770175	32.069466
611.592189	39664.932405	32.074484
612.589638	39727.633617	32.079501
612.896461	39794.862426	32.084519
613.294815	39852.984889	32.089536
614.260837	39919.808363	32.094554
614.372066	39988.569702	32.099572
615.033238	40063.295035	32.104589
615.832424	40141.678668	32.109607
616.173939	40213.464846	32.114624
616.735263	40282.392736	32.119642
617.306390	40359.669100	32.124660
618.026257	40433.309741	32.129677
618.603413	40509.935425	32.134695
619.263724	40594.793438	32.139712
620.022493	40659.418815	32.144730
620.488752	40739.305925	32.149748
621.066483	40805.956930	32.154765
621.973898	40889.342177	32.159783
622.220253	40973.029739	32.164800
623.137516	41042.943375	32.169818
623.658457	41113.585806	32.174836
624.624490	41190.089995	32.179853
624.931569	41258.249088	32.184871
625.571371	41335.988567	32.189888
626.291486	41408.512319	32.194906
626.957726	41483.798198	32.199924
627.604932	41544.893469	32.204941
628.084334	41621.382080	32.209959
628.972562	41707.823906	32.214976
629.943185	41764.304431	32.219994
630.101049	41840.982896	32.225012
630.996199	41910.395177	32.230029
631.422347	41986.954089	32.235047
632.315667	42052.591294	32.240064
632.834684	42116.437414	32.245082
633.396287	42189.037799	32.250100
633.928515	42246.312149	32.255117
634.563044	42311.140648	32.260135
634.745586	42387.555238	32.265152
635.759451	42454.408380	32.270170
636.261113	42516.089749	32.275188
636.788518	42581.167387	32.280205
637.685546	42651.311442	32.285223
638.207943	42721.745061	32.290240
639.067810	42795.087777	32.295258
639.381161	42872.991884	32.300276
639.954993	42933.980728	32.305293
640.668425	43006.173993	32.310311
641.156171	43089.925870	32.315328
641.708718	43159.175321	32.320346
642.317069	43234.114772	32.325364
642.854109	43312.785667	32.330381
643.916426	43391.107935	32.335399
644.210807	43470.889983	32.340416
645.061022	43549.469020	32.345434
645.900496	43617.608664	32.350452
646.503354	43696.737581	32.355469
647.487282	43764.904384	32.360487
647.452995	43857.867839	32.365504
648.456969	43924.153233	32.370522
648.931143	44003.386826	32.375540
649.508909	44087.270358	32.380557
650.627746	44162.268003	32.385575
650.984293	44242.447208	32.390592
651.703248	44313.709986	32.395610
652.263260	44399.710225	32.400628
652.705586	44475.373604	32.405645
653.287561	44563.783318	32.410663
654.081049	44651.583780	32.415680
654.855581	44724.108261	32.420698
655.565872	44817.647951	32.425716
656.018265	44900.314918	32.430733
656.616294	44987.783000	32.435751
657.386742	45074.515655	32.440768
658.514607	45146.642288	32.445786
659.178176	45230.671449	32.450804
659.965560	45304.244383	32.455821
660.306124	45388.993953	32.460839
660.561644	45471.544422	32.465856
661.249399	45549.985028	32.470874
662.065811	45632.399204	32.475892
662.765314	45730.015516	32.480909
663.540808	45807.230101	32.485927
663.709520	45906.583482	32.490944
665.049080	45980.152963	32.495962
665.781500	46075.122543	32.500980
666.441688	46157.921684	32.505997
667.427332	46234.083271	32.511015
667.520643	46318.388440	32.516032
668.606847	46391.180394	32.521050
669.009470	46470.906706	32.526068
669.846864	46550.877219	32.531085
670.833621	46623.945464	32.536103
671.041257	46709.146087	32.541120
671.765768	46786.698361	32.546138
672.335565	46865.669195	32.551156
673.062393	46960.524129	32.556173
674.109903	47037.430300	32.561191
674.608707	47119.000302	32.566208
675.438820	47191.645053	32.571226
675.991643	47263.069595	32.576244
676.552152	47348.454711	32.581261
677.362502	47420.014088	32.586279
677.788084	47508.201304	32.591296
678.407082	47580.674032	32.596314
679.053279	47655.631092	32.601332
679.672077	47738.977678	32.606349
680.346236	47812.225364	32.611367
680.757480	47890.301352	32.616384
681.611968	47951.032599	32.621402
681.955786	48039.892682	32.626420
682.603343	48123.694117	32.631437
683.308805	48209.867590	32.636455
683.636238	48297.954675	32.641472
684.645653	48380.677286	32.646490
685.174437	48478.812823	32.651508
685.536629	48569.775687	32.656525
686.441661	48654.632753	32.661543
687.208210	48762.707263	32.666560
688.036760	48842.786752	32.671578
688.971073	48936.754967	32.676596
689.276185	49039.317218	32.681613
690.409512	49118.084121	32.686631
690.721863	49219.764968	32.691648
691.365468	49305.451421	32.696666
692.484092	49392.114566	32.701684
693.160009	49487.432617	32.706701
694.007044	49573.484566	32.711719
694.217287	49667.756157	32.716736
695.365946	49755.837250	32.721754
695.901715	49850.652826	32.726772
696.615509	49940.461714	32.731789
697.470152	50032.941884	32.736807
698.132586	50133.678953	32.741824
698.635145	50217.365051	32.746842
699.736850	50305.734369	32.751860
699.863654	50400.001225	32.756877
700.798142	50487.571505	32.761895
701.862080	50593.813043	32.766912
702.498976	50677.573666	32.771930
703.357892	50769.712370	32.776948
703.887127	50858.785359	32.781965
704.695050	50946.245989	32.786983
704.941456	51034.892781	32.792000
705.728081	51134.783797	32.797018
706.899966	51227.820496	32.802036
706.969896	51324.558680	32.807053
707.615934	51420.431327	32.812071
708.478596	51513.981716	32.817088
709.208593	51608.944334	32.822106
709.899914	51702.328131	32.827124
710.308693	51808.918441	32.832141
711.173026	51909.084865	32.837159
711.822787	52020.633630	32.842176
712.794735	52111.104794	32.847194
713.600793	52213.790506	32.852212
713.955720	52331.720075	32.857229
714.859611	52421.123615	32.862247
715.439100	52519.596609	32.867264
716.704494	52624.735587	32.872282
717.450481	52721.305682	32.877300
717.846973	52805.728050	32.882317
718.832186	52901.930939	32.887335
719.578565	52997.763146	32.892352
719.940669	53093.318220	32.897370
720.926346	53196.042554	32.902388
721.532913	53287.622061	32.907405
722.520887	53388.963392	32.912423
723.111908	53483.616933	32.917440
723.648899	53567.930887	32.922458
724.540250	53670.338449	32.927476
725.256514	53769.420585	32.932493
725.922152	53849.645597	32.937511
726.567665	53932.673216	32.942528
727.272514	54026.653450	32.947546
727.994298	54117.232123	32.952564
728.722344	54200.089261	32.957581
730.235891	54281.755344	32.962599
730.774681	54369.307395	32.967616
730.926682	54457.947384	32.972634
731.829881	54538.786696	32.977652
732.316552	54631.674915	32.982669
733.396981	54730.076120	32.987687
734.041251	54816.475387	32.992704
734.654982	54906.728041	32.997722
735.447942	54994.057580	33.002740
735.692677	55097.969585	33.007757
736.711448	55186.728525	33.012775
737.441921	55284.703846	33.017792
738.203772	55389.732378	33.022810
738.687435	55482.087999	33.027828
739.373735	55593.695205	33.032845
739.957744	55696.833894	33.037863
741.076609	55796.156573	33.042880
741.699756	55905.646553	33.047898
742.394204	56003.808306	33.052916
742.890340	56107.387020	33.057933
744.091438	56212.467304	33.062951
744.659538	56316.686049	33.067968
745.688109	56424.468898	33.072986
746.692144	56521.886910	33.078004
747.156346	56633.366069	33.083021
748.275096	56730.860913	33.088039
748.861988	56832.248302	33.093056
749.347297	56924.085850	33.098074
750.431573	57017.802642	33.103092
750.731917	57129.564437	33.108109
752.048584	57226.946815	33.113127
753.041892	57326.752874	33.118144
753.616914	57421.497360	33.123162
754.728661	57504.216340	33.128180
755.241449	57620.255499	33.133197
755.759292	57712.306138	33.138215
756.566954	57803.146490	33.143232
757.252921	57906.899025	33.148250
758.394827	58011.530920	33.153268
759.112820	58109.522170	33.158285
759.739156	58211.415569	33.163303
760.254937	58298.129229	33.168320
761.026742	58413.232744	33.173338
762.042905	58508.440234	33.178356
762.701029	58617.111384	33.183373
763.478639	58712.871189	33.188391
764.198022	58814.878642	33.193408
764.663528	58916.302947	33.198426
765.749300	59019.925568	33.203444
766.370442	59128.611907	33.208461
766.905642	59228.850767	33.213479
767.980533	59333.292055	33.218496
768.469987	59443.607117	33.223514
769.624665	59542.146126	33.228532
769.945452	59657.268129	33.233549
770.573773	59755.585558	33.238567
771.789724	59861.870644	33.243584
772.277132	59973.863741	33.248602
773.023229	60069.407655	33.253620
773.622254	60180.587095	33.258637
774.674336	60293.398654	33.263655
775.834054	60398.943752	33.268672
776.647304	60502.138691	33.273690
777.666586	60576.606042	33.278708
778.019516	60675.883591	33.283725
778.321178	60767.490904	33.288743
779.542209	60851.760322	33.293760
779.942072	60963.204508	33.298778
780.947684	61054.734600	33.303796
781.245991	61162.644598	33.308813
782.335554	61267.428383	33.313831
782.904694	61363.254132	33.318848
783.602424	61479.316401	33.323866
784.482206	61577.373490	33.328884
785.193427	61695.425734	33.333901
785.998591	61797.016798	33.338919
786.732295	61908.720626	33.343936
787.476072	62024.064128	33.348954
788.316410	62125.227512	33.353972
789.076287	62246.296195	33.358989
789.509818	62339.121278	33.364007
790.602565	62461.431938	33.369024
791.142786	62582.387230	33.374042
792.017998	62701.208242	33.379060
793.048933	62813.424066	33.384077
793.893535	62928.193397	33.389095
795.160295	63042.817690	33.394112
795.762548	63165.580278	33.399130
796.654815	63268.371525	33.404148
797.463923	63377.694122	33.409165
798.529833	63489.345258	33.414183
799.077850	63599.173654	33.419200
799.555841	63710.044575	33.424218
800.656903	63812.500575	33.429236
801.433053	63935.757314	33.434253
802.127961	64050.785202	33.439271
803.319111	64162.356041	33.444288
804.069884	64275.555381	33.449306
804.711143	64387.483878	33.454324
805.656100	64495.247471	33.459341
806.502473	64611.125774	33.464359
807.284657	64716.957771	33.469376
807.729398	64846.216970	33.474394
808.998209	64956.786743	33.479412
809.774448	65067.482823	33.484429
810.231006	65180.451272	33.489447
811.089182	65300.750310	33.494464
811.697595	65414.763280	33.499482
813.206378	65534.500893	33.504500
813.774021	65650.077049	33.509517
814.422333	65760.993938	33.514535
815.514434	65869.182825	33.519552
816.051553	65996.423499	33.524570
816.771540	66109.277530	33.529588
817.637894	66231.818542	33.534605
818.434143	66351.507984	33.539623
819.458582	66463.270430	33.544640
819.770824	66597.291259	33.549658
821.015918	66711.914057	33.554676
821.469127	66829.051911	33.559693
822.218038	66951.780920	33.564711
823.269065	67071.192075	33.569728
824.001475	67194.589063	33.574746
825.095426	67307.128458	33.579764
826.175667	67431.961374	33.584781
826.724562	67549.751250	33.589799
827.576161	67669.268321	33.594816
828.201002	67778.359900	33.599834
829.035501	67902.654573	33.604852
830.236173	68026.870447	33.609869
830.994049	68138.647923	33.614887
831.607204	68237.273634	33.619904
832.050188	68358.904374	33.624922
833.397871	68476.187934	33.629940
834.254245	68574.111105	33.634957
834.933159	68681.731523	33.639975
835.660616	68791.418323	33.644992
836.546514	68909.185304	33.650010
837.237473	69020.839388	33.655028
838.026207	69143.587155	33.660045
838.819920	69273.694662	33.665063
839.680384	69381.326527	33.670080
840.368583	69495.904750	33.675098
841.305696	69628.229032	33.680116
841.944314	69745.371288	33.685133
842.464710	69874.876385	33.690151
843.788230	69995.586771	33.695168
844.535067	70126.440702	33.700186
845.607086	70241.996441	33.705204
846.420089	70358.638972	33.710221
847.207791	70491.195640	33.715239
848.338536	70607.837562	33.720256
849.405652	70742.398318	33.725274
850.104170	70863.197984	33.730292
851.082919	70980.271762	33.735309
851.961830	71106.841524	33.740327
852.802045	71223.642335	33.745344
853.734777	71358.077401	33.750362
854.624825	71472.443088	33.755380
855.578933	71589.568516	33.760397
856.187108	71724.413660	33.765415
857.328217	71831.220940	33.770432
857.536453	71960.353879	33.775450
858.627240	72091.352575	33.780468
859.627351	72215.878876	33.785485
860.369906	72356.466684	33.790503
861.402036	72477.036810	33.795520
862.135884	72609.122129	33.800538
863.175277	72737.451903	33.805556
864.035733	72864.857111	33.810573
864.835043	72990.224204	33.815591
865.769672	73106.519958	33.820608
866.659327	73243.541398	33.825626
868.032862	73363.294766	33.830644
869.646421	73456.346566	33.835661
870.344318	73581.759131	33.840679
871.918279	73673.155152	33.845696
872.812167	73789.398047	33.850714
873.756484	73881.955218	33.855732
874.502818	73978.232576	33.860749
875.615055	74082.684092	33.865767
876.111792	74175.000308	33.870784
876.920703	74287.041570	33.875802
877.675069	74391.041467	33.880820
878.548686	74498.310838	33.885837
879.149186	74591.737395	33.890855
880.110932	74705.216467	33.895872
881.074000	74820.707103	33.900890
881.678677	74928.491066	33.905908
882.474129	75037.414055	33.910925
882.924514	75158.816193	33.915943
883.750299	75277.715601	33.920960
884.460992	75392.175782	33.925978
885.013475	75519.773861	33.930996
886.248984	75636.906098	33.936013
886.939533	75769.087206	33.941031
887.912197	75897.667895	33.946048
888.692666	76031.106989	33.951066
889.394336	76148.538942	33.956084
890.609052	76257.809734	33.961101
891.277106	76383.723901	33.966119
892.174156	76495.350686	33.971136
892.483246	76610.705834	33.976154
893.561245	76735.504247	33.981172
894.227266	76856.026147	33.986189
894.977814	76987.097699	33.991207
895.971410	77114.650983	33.996224
896.914931	77236.356135	34.001242
897.652490	77377.514518	34.006260
898.375854	77515.026450	34.011277
899.302964	77649.602210	34.016295
900.446456	77777.646849	34.021312
901.082060	77925.713877	34.026330
901.803831	78067.587674	34.031348
902.903744	78209.285978	34.036365
903.476630	78352.716969	34.041383
904.468276	78486.837977	34.046400
905.769334	78626.532079	34.051418
906.433859	78767.837816	34.056436
907.818246	78907.589469	34.061453
909.016208	79051.762869	34.066471
909.556299	79183.059200	34.071488
910.378847	79322.956948	34.076506
911.396556	79467.820701	34.081524
913.044001	79600.441890	34.086541
913.694936	79743.476629	34.091559
914.842310	79875.100396	34.096576
915.948930	79995.243677	34.101594
916.520754	80135.396675	34.106612
917.998206	80270.029951	34.111629
918.713928	80409.819242	34.116647
919.535007	80538.717340	34.121664
920.819916	80665.572028	34.126682
921.392896	80803.362971	34.131700
922.469403	80922.883525	34.136717
923.150009	81069.913579	34.141735
923.962121	81193.521772	34.146752
925.153983	81332.548428	34.151770
926.284793	81477.381006	34.156788
927.099327	81595.423748	34.161805
927.801554	81746.832477	34.166823
928.626956	81882.962295	34.171840
929.704984	82032.874656	34.176858
930.445241	82170.361491	34.181876
931.821977	82304.966511	34.186893
932.525297	82445.459924	34.191911
933.479263	82577.257821	34.196928
934.509120	82710.208044	34.201946
935.106417	82855.238784	34.206964
936.125271	82986.844822	34.211981
937.267646	83135.279592	34.216999
938.116315	83276.310805	34.222016
938.770383	83416.698078	34.227034
939.757707	83560.770335	34.232052
940.751173	83697.629686	34.237069
941.567815	83846.742940	34.242087
942.560343	83989.450365	34.247104
943.533126	84130.346049	34.252122
944.314928	84283.941155	34.257140
945.201537	84425.979120	34.262157
946.426896	84572.618790	34.267175
947.312748	84712.456751	34.272192
948.512060	84857.710524	34.277210
949.192142	85004.202644	34.282228
950.542014	85136.006598	34.287245
951.294692	85283.209789	34.292263
952.308917	85425.764256	34.297280
953.137609	85563.693221	34.302298
954.116698	85687.766107	34.307316
955.143248	85819.690660	34.312333
955.866525	85956.171370	34.317351
956.759516	86081.431189	34.322368
957.834388	86214.634490	34.327386
958.595746	86348.023271	34.332404
959.648408	86481.953122	34.337421
960.482478	86620.532847	34.342439
961.129249	86760.992087	34.347456
962.320659	86903.317419	34.352474
963.231969	87047.854073	34.357492
964.605984	87192.403693	34.362509
965.146498	87346.071445	34.367527
965.880714	87488.418954	34.372544
966.818909	87631.613192	34.377562
967.665308	87781.556583	34.382580
968.688008	87924.346275	34.387597
970.091638	88083.261344	34.392615
971.032919	88235.128340	34.397632
971.742114	88393.065527	34.402650
972.487146	88532.544478	34.407668
973.591612	88691.544725	34.412685
974.751267	88854.637707	34.417703
975.507956	89010.387837	34.422720
976.894148	89160.548104	34.427738
977.932229	89320.373565	34.432756
979.031240	89462.849770	34.437773
979.958535	89626.214271	34.442791
980.726201	89778.600774	34.447808
982.196510	89929.973390	34.452826
983.143326	90094.736493	34.457844
984.276764	90228.319702	34.462861
985.232205	90377.710772	34.467879
985.869071	90536.876540	34.472896
987.308326	90690.480505	34.477914
988.155364	90841.721423	34.482932
989.331039	90992.579843	34.487949
990.211322	91149.747428	34.492967
990.899718	91306.555362	34.497984
992.303835	91455.106771	34.503002
992.828852	91612.779141	34.508020
993.876375	91765.606610	34.513037
995.100355	91928.089543	34.518055
996.023318	92088.794185	34.523072
996.923830	92247.123789	34.528090
997.944620	92406.586472	34.533108
998.623234	92564.562412	34.538125
999.990750	92725.704100	34.543143
1000.439236	92889.695157	34.548160
1001.800507	93053.909828	34.553178
1002.479782	93228.232708	34.558196
1003.996073	93392.360724	34.563213
1004.761261	93554.632859	34.568231
1005.199924	93731.689192	34.573248
1006.526158	93879.059283	34.578266
1007.503324	94053.326109	34.583284
1008.427420	94216.924578	34.588301
1009.125157	94382.568118	34.593319
1010.564424	94559.104154	34.598336
1011.225754	94735.744761	34.603354
1012.278693	94910.315278	34.608372
1013.164273	95085.250189	34.613389
1014.320585	95251.798553	34.618407
1015.080441	95440.917106	34.623424
1016.276238	95607.480319	34.628442
1017.500971	95789.953971	34.633460
1018.338629	95951.027120	34.638477
1019.644573	96121.057191	34.643495
1020.627457	96281.583052	34.648512
1021.665167	96439.157263	34.653530
1022.899738	96602.302324	34.658548
1023.646030	96756.394355	34.663565
1024.688211	96914.844426	34.668583
1025.781253	97087.739671	34.673600
1026.506993	97240.837856	34.678618
1027.745805	97407.241367	34.683636
1028.890449	97569.989776	34.688653
1029.892316	97725.824414	34.693671
1030.674990	97902.954835	34.698688
1031.781232	98056.159668	34.703706
1032.617009	98241.380738	34.708724
1033.887371	98413.388449	34.713741
1035.096229	98582.767515	34.718759
1035.618507	98756.553610	34.723776
1036.788399	98923.003836	34.728794
1037.813186	99103.299778	34.733812
1038.870070	99283.572699	34.738829
1040.169039	99453.620104	34.743847
1041.051169	99647.118542	34.748864
1042.257911	99811.213297	34.753882
1043.001522	100002.002248	34.758900
1043.931727	100176.661284	34.763917
1045.353211	100356.754882	34.768935
1045.923661	100546.557177	34.773952
1047.979258	100706.819803	34.778970
1048.861250	100909.584357	34.783988
1049.645748	101094.619370	34.789005
1050.476185	101261.786772	34.794023
1051.568841	101443.822836	34.799040
1052.669604	101626.903567	34.804058
1053.628755	101819.316605	34.809076
1054.301889	102012.316561	34.814093
1055.739865	102192.838175	34.819111
1056.391431	102380.595387	34.824128
1057.446536	102577.006240	34.829146
1058.523760	102772.078883	34.834164
1059.714551	102962.644839	34.839181
1060.987314	103158.080629	34.844199
1062.333006	103357.330398	34.849216
1063.290139	103545.843332	34.854234
1064.111624	103734.557352	34.859252
1065.706417	103927.476112	34.864269
1066.760565	104106.592708	34.869287
1067.889921	104308.608356	34.874304
1069.274522	104494.803141	34.879322
1070.427309	104675.224435	34.884340
1071.417963	104862.120189	34.889357
1072.465056	105048.058065	34.894375
1073.248623	105239.360140	34.899392
1074.442514	105415.144288	34.904410
1075.373507	105603.359658	34.909428
1076.050197	105796.190586	34.914445
1077.737791	105974.556540	34.919463
1078.404547	106176.599622	34.924480
1079.274131	106362.601397	34.929498
1080.559037	106552.170855	34.934516
1081.337538	106763.813165	34.939533
1082.411365	106942.084421	34.944551
1083.440775	107150.445849	34.949568
1084.246204	107345.698561	34.954586
1085.476221	107549.913463	34.959604
1086.314992	107759.083772	34.964621
1088.070799	107955.007098	34.969639
1088.800076	108157.384115	34.974656
1089.985123	108347.565432	34.979674
1091.452321	108538.651440	34.984692
1092.450546	108727.054991	34.989709
1093.710566	108903.965796	34.994727
1094.575489	109089.391877	34.999744
1095.802508	109262.421749	35.004762
1096.810228	109451.006098	35.009780
1097.828952	109634.801761	35.014797
1098.937745	109804.485172	35.019815
1100.035931	110010.792533	35.024832
1101.187423	110195.152720	35.029850
1102.718034	110381.224920	35.034868
1103.137420	110570.433637	35.039885
1104.639269	110756.069775	35.044903
1105.403177	110954.408226	35.049920
1106.655635	111136.528534	35.054938
1107.862683	111331.946188	35.059956
1108.863201	111526.917989	35.064973
1110.207132	111722.125760	35.069991
1111.033564	111918.687282	35.075008
1112.263309	112106.328407	35.080026
1113.292481	112307.115707	35.085044
1114.238682	112508.222220	35.090061
1115.383784	112704.761969	35.095079
1116.816313	112911.289145	35.100096
1117.863114	113105.795660	35.105114
1119.143616	113305.763159	35.110132
1120.222658	113515.634471	35.115149
1121.454621	113718.248078	35.120167
1122.149785	113909.676408	35.125184
1123.585964	114113.259968	35.130202
1124.491865	114314.310131	35.135220
1125.761180	114527.704954	35.140237
1126.905871	114723.802854	35.145255
1127.982159	114939.943970	35.150272
1129.020868	115148.921935	35.155290
1130.376443	115357.342271	35.160308
1131.630548	115557.190775	35.165325
1132.697936	115761.835441	35.170343
1134.136306	115975.656686	35.175360
1135.265672	116179.749304	35.180378
1136.044761	116387.284229	35.185396
1137.143518	116592.436485	35.190413
1138.174456	116803.341103	35.195431
1139.349913	117010.992416	35.200448
1140.537981	117226.676282	35.205466
1141.818756	117433.996482	35.210484
1142.384127	117657.731024	35.215501
1143.938877	117864.933011	35.220519
1145.071440	118090.059632	35.225536
1146.153747	118300.421886	35.230554
1147.429552	118510.373548	35.235572
1148.340276	118732.918919	35.240589
1149.452086	118948.374830	35.245607
1150.556595	119172.336062	35.250624
1152.092190	119393.363991	35.255642
1153.210606	119605.034888	35.260660
1153.950796	119824.474232	35.265677
1155.401568	120045.026920	35.270695
1156.582371	120276.815174	35.275712
1158.006325	120498.313424	35.280730
1159.437251	120701.323628	35.285748
1160.322211	120923.218308	35.290765
1161.515222	121138.258726	35.295783
1162.489702	121351.347276	35.300800
1163.504854	121563.176064	35.305818
1165.036319	121779.913995	35.310836
1165.701866	122006.846048	35.315853
1167.097028	122219.212313	35.320871
1168.093333	122425.778514	35.325888
1169.115035	122635.611556	35.330906
1170.551922	122847.253041	35.335924
1171.179553	123054.784318	35.340941
1172.365397	123255.216495	35.345959
1173.500861	123469.953765	35.350976
1174.248033	123686.049437	35.355994
1175.574139	123907.094986	35.361012
1176.940089	124133.927372	35.366029
1178.363753	124355.606430	35.371047
1179.509006	124573.163482	35.376064
1180.666626	124798.324337	35.381082
1181.543400	125017.741312	35.386100
1182.672933	125253.214063	35.391117
1183.599777	125485.807096	35.396135
1185.131993	125715.133283	35.401152
1185.913060	125957.513132	35.406170
1187.380883	126176.156321	35.411188
1188.114324	126431.234844	35.416205
1189.538080	126658.241237	35.421223
1190.622714	126903.645618	35.426240
1191.792986	127144.855117	35.431258
1193.102874	127394.091969	35.436276
1193.964202	127642.733199	35.441293
1195.236327	127879.938967	35.446311
1196.797244	128131.472461	35.451328
1197.614698	128382.002781	35.456346
1199.114950	128628.277395	35.461364
1200.376237	128888.637888	35.466381
1201.540568	129128.697601	35.471399
1202.581748	129389.428199	35.476416
1203.679384	129636.081496	35.481434
1205.232190	129882.623457	35.486452
1206.427598	130151.523491	35.491469
1207.633090	130397.695897	35.496487
1209.036868	130656.551662	35.501504
1210.334163	130906.807255	35.506522
1211.961461	131154.994719	35.511540
1212.767243	131403.763586	35.516557
1214.047722	131648.158559	35.521575
1215.515538	131910.601394	35.526592
1216.365268	132164.591705	35.531610
1218.151600	132411.178022	35.536628
1219.221178	132667.531894	35.541645
1220.478466	132919.774750	35.546663
1221.875426	133166.672066	35.551680
1222.793704	133418.670592	35.556698
1224.602507	133674.365123	35.561716
1225.432013	133916.772725	35.566733
1226.473325	134161.441759	35.571751
1227.502984	134408.041556	35.576768
1228.695510	134672.529980	35.581786
1230.540309	134928.076243	35.586804
1231.326444	135186.068838	35.591821
1232.628859	135439.477400	35.596839
1234.342776	135703.507587	35.601856
1235.135564	135949.688995	35.606874
1236.127233	136204.726887	35.611892
1237.558482	136463.180654	35.616909
1238.714574	136717.079593	35.621927
1240.251064	136981.288727	35.626944
1241.135148	137232.852958	35.631962
1242.791882	137495.588222	35.636980
1243.772932	137750.982002	35.641997
1245.278414	137991.913006	35.647015
1246.646246	138254.968212	35.652032
1247.357405	138512.200124	35.657050
1249.035426	138760.538122	35.662068
1249.951416	139013.555804	35.667085
1251.399146	139243.715077	35.672103
1253.042095	139491.620431	35.677120
1253.874728	139721.047739	35.682138
1255.300664	139957.225597	35.687156
1256.615494	140202.438826	35.692173
1258.120376	140437.174115	35.697191
1258.944281	140668.549231	35.702208
1259.882834	140920.245863	35.707226
1261.413301	141162.044687	35.712244
1262.636048	141414.192467	35.717261
1263.899433	141660.679905	35.722279
1265.236644	141913.142077	35.727296
1266.467797	142176.135809	35.732314
1267.553352	142411.663886	35.737332
1268.756304	142667.704288	35.742349
1270.023148	142926.462382	35.747367
1271.440165	143179.770114	35.752384
1272.172268	143445.392028	35.757402
1273.501978	143707.252318	35.762420
1275.021221	143970.211846	35.767437
1276.146092	144243.776686	35.772455
1277.410373	144511.740760	35.777472
1278.209931	144783.156941	35.782490
1279.804874	145043.943346	35.787508
1280.944549	145327.748101	35.792525
1282.585156	145607.743853	35.797543
1283.667960	145878.474729	35.802560
1284.738026	146158.721240	35.807578
1286.437484	146434.756897	35.812596
1287.495048	146714.299573	35.817613
1288.711288	147001.554370	35.822631
1290.141551	147284.958656	35.827648
1291.459543	147568.688075	35.832666
1292.808132	147849.370812	35.837684
1293.930969	148128.571081	35.842701
1295.087510	148418.649723	35.847719
1296.708307	148706.497822	35.852736
1297.845581	149001.949082	35.857754
1299.487715	149264.343246	35.862772
1300.648835	149562.496512	35.867789
1301.865650	149852.753958	35.872807
1303.285459	150130.994321	35.877824
1304.807172	150422.106303	35.882842
1306.351313	150706.253556	35.887860
1307.652786	150995.161377	35.892877
1308.866769	151273.735920	35.897895
1310.387085	151556.130454	35.902912
1311.817117	151848.093014	35.907930
1312.925149	152130.762891	35.912948
1314.331199	152409.935521	35.917965
1315.443031	152702.705559	35.922983
1317.263632	152975.699994	35.928000
1318.416220	153268.695918	35.933018
1319.980467	153542.447058	35.938036
1321.273363	153830.806891	35.943053
1322.553668	154109.581320	35.948071
1324.073062	154382.508603	35.953088
1325.156133	154663.501367	35.958106
1326.463901	154951.575273	35.963124
1327.930786	155223.020265	35.968141
1329.012598	155510.425243	35.973159
1330.686103	155788.055695	35.978176
1331.797584	156071.197608	35.983194
1333.206787	156346.402013	35.988212
1334.297126	156633.927890	35.993229
1335.520431	156910.105634	35.998247
1336.991345	157189.326980	36.003264
1338.082505	157469.830860	36.008282
1339.373585	157737.376776	36.013300
1340.669202	158009.757054	36.018317
1341.634708	158291.467198	36.023335
1343.132814	158559.517145	36.028352
1344.551040	158840.268247	36.033370
1345.518362	159106.975973	36.038388
1346.785998	159400.746555	36.043405
1348.327380	159682.256945	36.048423
1349.532790	159960.183748	36.053440
1350.611933	160262.263248	36.058458
1352.067190	160562.113363	36.063476
1353.597077	160845.257470	36.068493
1354.707182	161139.688088	36.073511
1355.950644	161431.282231	36.078528
1357.457947	161734.164355	36.083546
1358.594682	162044.024407	36.088564
1359.997269	162350.074683	36.093581
1361.181085	162653.765417	36.098599
1362.434008	162960.606074	36.103616
1363.661342	163279.316015	36.108634
1365.376948	163588.241605	36.113652
1366.654367	163906.364305	36.118669
1367.949326	164230.195976	36.123687
1369.677216	164531.881570	36.128704
1370.517551	164861.401151	36.133722
1372.017300	165178.862069	36.138740
1373.659936	165499.372227	36.143757
1374.917919	165828.297187	36.148775
1376.454294	166144.223774	36.153792
1378.109275	166474.838957	36.158810
1379.297979	166788.683258	36.163828
1380.494566	167112.742837	36.168845
1381.841978	167439.038445	36.173863
1383.452508	167770.876041	36.178880
1385.022779	168101.491918	36.183898
1386.535026	168413.276616	36.188916
1387.930062	168742.010104	36.193933
1389.200564	169073.951545	36.198951
1391.063647	169388.324324	36.203968
1392.559089	169716.667580	36.208986
1393.925762	170029.312215	36.214004
1395.383734	170349.570308	36.219021
1396.628843	170666.680698	36.224039
1398.425328	170985.250288	36.229056
1399.461517	171315.838059	36.234074
1401.167300	171637.294994	36.239092
1402.722497	171946.964638	36.244109
1403.753854	172279.780752	36.249127
1405.664344	172603.520058	36.254144
1406.904091	172912.740556	36.259162
1408.210223	173232.243953	36.264180
1409.726146	173558.935669	36.269197
1410.848897	173881.976263	36.274215
1412.321485	174203.793682	36.279232
1413.724427	174520.104311	36.284250
1415.250897	174843.046547	36.289268
1416.863555	175167.664565	36.294285
1417.880552	175494.794446	36.299303
1419.596059	175811.302927	36.304320
1420.891181	176140.840513	36.309338
1422.158409	176474.636448	36.314356
1423.757699	176795.955011	36.319373
1425.183918	177123.078806	36.324391
1426.646453	177439.537941	36.329408
1428.446046	177778.458105	36.334426
1429.377324	178087.597260	36.339444
1430.779014	178399.998477	36.344461
1432.218872	178723.894025	36.349479
1433.630664	179031.525350	36.354496
1435.043430	179329.220606	36.359514
1436.180133	179643.868905	36.364532
1437.616780	179957.720727	36.369549
1438.860766	180277.926963	36.374567
1440.257540	180590.849980	36.379584
1441.447465	180914.813257	36.384602
1442.462153	181236.890942	36.389620
1444.144209	181571.654296	36.394637
1445.009462	181910.007099	36.399655
1446.520755	182239.103939	36.404672
1447.848374	182594.291228	36.409690
1449.516919	182938.127972	36.414708
1450.747338	183280.947720	36.419725
1452.106437	183643.219324	36.424743
1453.331814	184001.415592	36.429760
1454.846218	184364.453289	36.434778
1456.321547	184729.670375	36.439796
1458.208535	185098.058638	36.444813
1459.295205	185469.196418	36.449831
1460.965698	185829.590408	36.454848
1462.486608	186195.203079	36.459866
1463.871116	186564.712207	36.464884
1465.695548	186932.665895	36.469901
1466.818905	187298.452926	36.474919
1468.203047	187673.046811	36.479936
1469.867431	188049.094713	36.484954
1471.214866	188419.485129	36.489972
1473.043242	188786.396421	36.494989
1474.223385	189167.406098	36.500007
1475.605209	189537.226676	36.505024
1477.286926	189918.031387	36.510042
1478.802034	190302.242782	36.515060
1480.456681	190677.357030	36.520077
1481.897943	191059.554365	36.525095
1483.335146	191436.384950	36.530112
1485.103980	191815.422740	36.535130
1486.701753	192204.202673	36.540148
1488.123344	192574.365387	36.545165
1489.002082	192966.823502	36.550183
1490.629276	193340.574883	36.555200
1492.259633	193724.763363	36.560218
1493.758219	194126.787325	36.565236
1495.743782	194503.025441	36.570253
1496.703685	194892.752669	36.575271
1498.372010	195274.417880	36.580288
1499.919976	195666.756765	36.585306
1501.617274	196056.381887	36.590324
1503.661509	196436.392185	36.595341
1504.844333	196826.271936	36.600359
1506.438195	197216.466949	36.605376
1507.833797	197590.573244	36.610394
1509.180203	197979.759849	36.615412
1510.838178	198355.058562	36.620429
1512.232509	198743.708417	36.625447
1513.691046	199139.548604	36.630464
1515.288183	199522.849683	36.635482
1516.493596	199929.667691	36.640500
1518.444379	200307.214033	36.645517
1519.803770	200699.232502	36.650535
1521.406327	201091.606566	36.655552
1522.903104	201484.622408	36.660570
1524.381363	201873.847170	36.665588
1526.039055	202264.174399	36.670605
1527.589418	202660.044570	36.675623
1529.172596	203048.052108	36.680640
1530.595916	203424.749747	36.685658
1531.904895	203801.392013	36.690676
1533.507961	204172.578648	36.695693
1534.582267	204546.368509	36.700711
1536.573980	204925.138311	36.705728
1537.851338	205299.317344	36.710746
1539.073967	205686.306132	36.715764
1540.708380	206062.017048	36.720781
1542.423485	206442.935094	36.725799
1543.751733	206833.099196	36.730816
1545.320541	207230.678950	36.735834
1546.888329	207613.620505	36.740852
1548.446825	208003.930080	36.745869
1549.722966	208400.243433	36.750887
1551.252656	208796.796178	36.755904
1552.774122	209197.669474	36.760922
1554.301471	209609.489356	36.765940
1556.019825	210013.864089	36.770957
1557.102410	210414.384011	36.775975
1558.833465	210819.243030	36.780992
1560.286634	211230.956097	36.786010
1561.678281	211652.992257	36.791028
1563.867702	212052.879825	36.796045
1565.027019	212476.304364	36.801063
1566.396183	212906.451814	36.806080
1568.528078	213324.030820	36.811098
1569.812160	213750.336033	36.816116
1571.361161	214170.707327	36.821133
1573.095100	214596.358025	36.826151
1574.638788	215015.845137	36.831168
1576.535440	215442.514110	36.836186
1577.779809	215873.788150	36.841204
1579.531875	216298.173661	36.846221
1581.501855	216732.760378	36.851239
1583.061256	217167.899422	36.856256
1584.679959	217582.585127	36.861274
1586.121497	218007.384910	36.866292
1587.678830	218441.615524	36.871309
1589.741819	218873.859575	36.876327
1591.213741	219313.670253	36.881344
1592.716537	219726.021779	36.886362
1594.302600	220161.245415	36.891380
1595.976255	220580.963079	36.896397
1597.782081	221014.528360	36.901415
1599.220691	221449.375188	36.906432
1601.159916	221874.413168	36.911450
1602.403481	222305.561911	36.916468
1603.944246	222737.983972	36.921485
1605.504769	223173.858730	36.926503
1607.627763	223614.391924	36.931520
1609.237555	224032.888506	36.936538
1610.675197	224522.838958	36.941556
1612.050601	224977.165767	36.946573
1614.020289	225407.215402	36.951591
1615.587357	225844.826045	36.956608
1617.093130	226267.335308	36.961626
1618.856866	226712.587306	36.966644
1620.790695	227133.225320	36.971661
1622.386610	227567.154086	36.976679
1623.994490	228003.266739	36.981696
1625.512981	228430.861019	36.986714
1627.142417	228858.158915	36.991732
1628.962620	229283.800985	36.996749
1630.408211	229721.495378	37.001767
1632.066612	230159.536982	37.006784
1633.808577	230586.161123	37.011802
1635.231118	231013.347298	37.016820
1637.300914	231443.729915	37.021837
1638.838848	231867.495734	37.026855
1640.044968	232283.595587	37.031872
1641.731810	232686.433907	37.036890
1643.182729	233108.109183	37.041908
1645.025604	233513.946578	37.046925
1646.540760	233930.990343	37.051943
1647.646742	234356.409033	37.056960
1649.502234	234769.537644	37.061978
1651.041030	235192.041955	37.066996
1652.568431	235619.451693	37.072013
1654.196436	236052.942254	37.077031
1655.350637	236487.070956	37.082048
1657.507831	236925.302508	37.087066
1658.792852	237375.592645	37.092084
1660.734301	237808.425856	37.097101
1662.495310	238248.656414	37.102119
1663.455680	238699.257227	37.107136
1665.596514	239137.318596	37.112154
1666.899791	239597.593730	37.117172
1668.902166	240049.219215	37.122189
1670.834998	240506.598032	37.127207
1672.049154	240968.389482	37.132224
1674.068489	241419.303638	37.137242
1675.177823	241882.841562	37.142260
1676.906033	242358.801564	37.147277
1678.807677	242810.144163	37.152295
1679.972311	243293.819758	37.157312
1682.126634	243768.213209	37.162330
1683.851655	244239.172820	37.167348
1685.599783	244715.946612	37.172365
1687.211539	245187.637749	37.177383
1688.706889	245686.453619	37.182400
1690.361011	246148.460752	37.187418
1692.027434	246635.081877	37.192436
1693.906238	247128.629008	37.197453
1696.054468	247598.355174	37.202471
1697.294910	248081.873269	37.207488
1699.261990	248567.151763	37.212506
1701.062770	249048.393819	37.217524
1702.779154	249536.026522	37.222541
1704.812813	250022.591221	37.227559
1706.233585	250510.858045	37.232576
1708.293792	250992.110071	37.237594
1709.744941	251482.684470	37.242612
1711.746164	251970.551903	37.247629
1713.513638	252449.186166	37.252647
1715.268240	252930.998299	37.257664
1717.472286	253412.761921	37.262682
1718.810831	253900.232102	37.267700
1720.649615	254376.950563	37.272717
1722.410597	254869.457536	37.277735
1724.067189	255351.642837	37.282752
1725.733522	255839.669469	37.287770
1727.297689	256320.524003	37.292788
1728.954718	256812.845617	37.297805
1731.235811	257305.216679	37.302823
1732.661376	257793.486771	37.307840
1734.457209	258280.425587	37.312858
1736.052368	258774.383474	37.317876
1737.752624	259262.023971	37.322893
1740.192620	259739.330122	37.327911
1741.398555	260236.832426	37.332928
1743.241858	260716.955121	37.337946
1745.036437	261210.422466	37.342964
1746.539026	261696.799561	37.347981
1748.542503	262178.216319	37.352999
1749.836785	262674.687119	37.358016
1751.815381	263166.929323	37.363034
1753.474256	263654.549867	37.368052
1755.345553	264121.837867	37.373069
1757.108502	264589.118063	37.378087
1758.567972	265066.660137	37.383104
1760.478818	265530.206369	37.388122
1762.061290	266001.706845	37.393140
1763.510496	266474.905533	37.398157
1765.821417	266956.928756	37.403175
1767.324526	267440.609105	37.408192
1768.869170	267922.478470	37.413210
1770.414572	268409.732615	37.418228
1772.160235	268893.015654	37.423245
1773.973417	269384.212669	37.428263
1775.476880	269881.201256	37.433280
1777.057483	270382.723533	37.438298
1779.201182	270889.486679	37.443316
1780.602108	271383.111465	37.448333
1782.521246	271891.256486	37.453351
1783.965319	272412.993366	37.458368
1785.755560	272925.298570	37.463386
1787.670098	273443.348718	37.468404
1789.504882	273968.599988	37.473421
1791.278767	274488.576552	37.478439
1792.788236	275016.622911	37.483456
1794.778509	275538.898602	37.488474
1796.571573	276070.096554	37.493492
1798.801339	276600.967153	37.498509
1800.607554	277137.164720	37.503527
1802.038477	277665.421276	37.508544
1804.004167	278200.777009	37.513562
1805.948211	278747.032414	37.518580
1807.547775	279287.526185	37.523597
1809.240547	279823.125917	37.528615
1811.322094	280370.116176	37.533632
1812.962957	280917.711054	37.538650
1814.797848	281461.817621	37.543668
1816.527280	282015.338536	37.548685
1818.452856	282563.948209	37.553703
1820.173079	283115.841412	37.558720
1822.251997	283670.543900	37.563738
1824.213609	284227.245169	37.568756
1826.423235	284774.860717	37.573773
1828.282435	285325.986758	37.578791
1829.928445	285874.859929	37.583808
1831.755441	286425.911076	37.588826
1833.474650	286979.289425	37.593844
1835.645158	287535.867806	37.598861
1837.531711	288087.182159	37.603879
1839.056192	288644.650227	37.608896
1840.881956	289198.992807	37.613914
1843.049741	289754.521215	37.618932
1844.806314	290319.995842	37.623949
1846.922204	290864.529796	37.628967
1848.672461	291422.685360	37.633984
1850.467971	291977.808366	37.639002
1852.519423	292538.169727	37.644020
1854.405919	293096.955543	37.649037
1856.318389	293644.279265	37.654055
1857.922215	294210.497707	37.659072
1860.267279	294767.548821	37.664090
1862.371367	295324.332189	37.669108
1863.449095	295881.510846	37.674125
1865.330514	296433.194794	37.679143
1867.340585	296984.168911	37.684160
1869.552252	297546.383853	37.689178
1871.215860	298100.482584	37.694196
1873.237231	298667.929572	37.699213
1874.849822	299204.988497	37.704231
1876.822965	299759.687443	37.709248
1878.723377	300295.423072	37.714266
1880.715464	300824.207043	37.719284
1882.264528	301363.245721	37.724301
1883.927926	301889.614535	37.729319
1885.454408	302424.104767	37.734336
1887.998420	302972.417753	37.739354
1890.022228	303509.994237	37.744372
1891.186675	304065.588844	37.749389
1893.035810	304601.359101	37.754407
1894.958707	305154.104243	37.759424
1896.715471	305713.070053	37.764442
1898.796915	306263.191546	37.769460
1900.344726	306827.568628	37.774477
1902.489193	307383.005650	37.779495
1904.130102	307947.918554	37.784512
1906.236955	308515.925104	37.789530
1908.305717	309084.924416	37.794548
1909.868618	309659.437825	37.799565
1912.026464	310229.836453	37.804583
1913.921307	310816.196946	37.809600
1915.699429	311384.364362	37.814618
1917.746739	311967.745215	37.819636
1919.360085	312552.742323	37.824653
1921.395434	313132.357869	37.829671
1923.241687	313717.180494	37.834688
1925.080746	314314.112457	37.839706
1927.364505	314904.211472	37.844724
1929.041019	315506.239195	37.849741
1931.644665	316107.143842	37.854759
1933.174845	316705.503619	37.859776
1935.083952	317302.018249	37.864794
1936.837950	317906.780496	37.869812
1938.375708	318512.995092	37.874829
1940.971305	319118.547180	37.879847
1943.042960	319726.541765	37.884864
1944.788905	320353.069561	37.889882
1947.064130	320950.685009	37.894900
1949.044206	321563.197451	37.899917
1950.990536	322171.469423	37.904935
1952.698309	322782.999610	37.909952
1954.899470	323401.805620	37.914970
1956.862422	324013.180220	37.919988
1958.571281	324633.553360	37.925005
1960.661555	325245.224869	37.930023
1963.011121	325856.745897	37.935040
1964.887041	326486.466687	37.940058
1966.930302	327084.696642	37.945076
1968.661247	327713.844509	37.950093
1970.533268	328323.946634	37.955111
1972.883889	328947.850562	37.960128
1974.695981	329572.445995	37.965146
1976.794659	330185.613786	37.970164
1978.701986	330813.480305	37.975181
1980.363756	331442.319699	37.980199
1982.862777	332060.529167	37.985216
1984.655747	332692.328409	37.990234
1986.541379	333318.875599	37.995252
1988.669325	333943.014725	38.000269
1990.546482	334564.217974	38.005287
1992.527081	335197.810247	38.010304
1994.481069	335832.313225	38.015322
1996.970620	336458.292520	38.020340
1998.747924	337091.743325	38.025357
2000.672186	337711.556412	38.030375
2002.441086	338344.587127	38.035392
2004.445354	338967.773229	38.040410
2006.805190	339593.964302	38.045428
2008.627073	340218.383471	38.050445
2010.768213	340823.806957	38.055463
2012.753314	341418.410715	38.060480
2014.430087	342030.292336	38.065498
2016.475114	342639.618129	38.070516
2018.236044	343241.927249	38.075533
2020.238114	343855.864144	38.080551
2022.240527	344477.559491	38.085568
2023.768564	345097.218470	38.090586
2025.982437	345702.695723	38.095604
2028.021561	346339.359847	38.100621
2029.944896	346966.694887	38.105639
2032.056773	347585.792960	38.110656
2033.858566	348232.164789	38.115674
2035.784812	348863.051713	38.120692
2037.913153	349516.025719	38.125709
2039.645412	350156.823783	38.130727
2041.954833	350798.329397	38.135744
2043.573036	351456.409151	38.140762
2045.828115	352105.213125	38.145780
2047.883070	352770.915329	38.150797
2049.824885	353439.797884	38.155815
2051.911602	354106.793735	38.160832
2053.602522	354772.423527	38.165850
2055.809341	355454.171756	38.170868
2058.130218	356128.963085	38.175885
2060.037434	356816.929796	38.180903
2062.187133	357499.745120	38.185920
2064.139142	358183.951873	38.190938
2065.973381	358870.906803	38.195956
2067.797664	359579.366864	38.200973
2069.957603	360276.494290	38.205991
2071.817192	360981.118151	38.211008
2073.943794	361688.577661	38.216026
2076.214993	362397.801888	38.221044
2078.186047	363118.073126	38.226061
2080.308986	363829.629833	38.231079
2082.624298	364539.924019	38.236096
2084.324148	365262.990633	38.241114
2086.599765	365982.676110	38.246132
2088.592079	366710.385280	38.251149
2090.670937	367436.924615	38.256167
2092.812352	368161.663897	38.261184
2094.810986	368906.755704	38.266202
2097.268551	369626.214221	38.271220
2099.057809	370367.379444	38.276237
2100.633678	371107.879988	38.281255
2103.026525	371856.854069	38.286272
2104.584826	372615.334561	38.291290
2106.794099	373357.129892	38.296308
2109.524967	374119.797800	38.301325
2111.232269	374866.716669	38.306343
2113.567691	375626.855639	38.311360
2115.463371	376383.829847	38.316378
2117.610931	377146.096763	38.321396
2119.867999	377907.720060	38.326413
2121.818879	378670.441946	38.331431
2123.863451	379432.979054	38.336448
2126.016045	380201.085024	38.341466
2128.121499	380981.073432	38.346484
2129.728049	381755.395416	38.351501
2131.946461	382530.942095	38.356519
2134.230374	383311.809522	38.361536
2136.516678	384087.663064	38.366554
2138.464899	384862.818585	38.371572
2140.613588	385659.117525	38.376589
2142.681680	386448.285929	38.381607
2144.947229	387242.092244	38.386624
2146.824687	388013.456204	38.391642
2148.682135	388776.413499	38.396660
2151.023724	389538.613149	38.401677
2153.247425	390311.815147	38.406695
2155.195986	391074.751633	38.411712
2157.199251	391850.891799	38.416730
2159.001504	392611.456755	38.421748
2161.269770	393392.557981	38.426765
2163.014196	394191.721155	38.431783
2165.207385	394967.623256	38.436800
2167.135098	395779.487814	38.441818
2169.280609	396575.961038	38.446836
2171.686411	397382.177637	38.451853
2173.683792	398183.725718	38.456871
2175.893463	398982.200998	38.461888
2177.707118	399815.513130	38.466906
2180.046344	400623.323207	38.471924
2182.147884	401446.049493	38.476941
2184.069109	402280.767106	38.481959
2186.650893	403100.553488	38.486976
2188.550809	403952.480491	38.491994
2190.612444	404791.863812	38.497012
2192.747964	405627.535859	38.502029
2195.250893	406493.549573	38.507047
2197.420486	407335.649973	38.512064
2199.671238	408200.435266	38.517082
2201.834155	409053.579741	38.522100
2204.058070	409913.906800	38.527117
2206.316805	410773.896551	38.532135
2208.396680	411650.023543	38.537152
2210.837037	412517.678024	38.542170
2213.000933	413382.816715	38.547188
2215.512429	414259.343008	38.552205
2217.356638	415135.139501	38.557223
2219.999195	416010.394753	38.562240
2222.190425	416892.228693	38.567258
2224.201678	417767.376358	38.572276
2226.912364	418645.974481	38.577293
2229.178970	419528.869642	38.582311
2231.948796	420403.522540	38.587328
2234.344842	421285.524336	38.592346
2236.579474	422156.785897	38.597364
2239.055256	423034.408091	38.602381
2241.157302	423899.148457	38.607399
2243.385206	424774.572100	38.612416
2245.272564	425662.121762	38.617434
2247.777982	426530.752900	38.622452
2250.130145	427418.212085	38.627469
2252.425530	428296.636200	38.632487
2254.637949	429173.371064	38.637504
2256.994770	430061.085655	38.642522
2259.088762	430951.847570	38.647540
2261.357752	431837.788614	38.652557
2263.426501	432725.045205	38.657575
2265.824304	433614.946909	38.662592
2267.851685	434515.048900	38.667610
2270.434926	435406.065685	38.672628
2272.800468	436296.071540	38.677645
2274.419111	437203.321959	38.682663
2276.913730	438095.766441	38.687680
2279.052684	438994.610390	38.692698
2281.511631	439902.929267	38.697716
2283.814375	440800.054440	38.702733
2285.876967	441711.147970	38.707751
2288.312620	442619.157247	38.712768
2290.557808	443524.377828	38.717786
2293.069371	444430.377060	38.722804
2295.620036	445322.318913	38.727821
2297.141989	446226.281803	38.732839
2299.677953	447101.661237	38.737856
2301.861334	447984.751768	38.742874
2304.082687	448874.729107	38.747892
2306.481509	449746.279788	38.752909
2308.160053	450647.854844	38.757927
2311.008829	451524.972984	38.762944
2312.738219	452416.399414	38.767962
2314.755235	453327.058117	38.772980
2317.098663	454232.161671	38.777997
2319.065456	455147.148052	38.783015
2321.598783	456048.398652	38.788032
2323.545139	456977.565683	38.793050
2325.929487	457905.354085	38.798068
2328.017943	458831.278261	38.803085
2330.208633	459783.178519	38.808103
2332.604068	460719.278246	38.813120
2334.796297	461676.092934	38.818138
2337.230676	462634.843514	38.823156
2339.817992	463585.233109	38.828173
2341.554629	464548.201123	38.833191
2344.029971	465512.869913	38.838208
2346.845655	466485.369164	38.843226
2349.004923	467464.952320	38.848244
2351.363955	468433.891680	38.853261
2353.321405	469424.828776	38.858279
2356.114243	470412.292489	38.863296
2358.414460	471410.547930	38.868314
2360.390406	472414.816365	38.873332
2363.496831	473400.001314	38.878349
2365.451219	474403.257872	38.883367
2367.704763	475399.793964	38.888384
2370.622857	476400.763477	38.893402
2372.877307	477409.667594	38.898420
2375.957565	478410.703423	38.903437
2378.119475	479417.037873	38.908455
2380.802049	480415.655993	38.913472
2383.591791	481414.908488	38.918490
2385.925986	482413.625494	38.923508
2388.181300	483418.510522	38.928525
2390.382491	484424.408382	38.933543
2393.063901	485424.717844	38.938560
2395.576960	486418.234044	38.943578
2398.179205	487425.561629	38.948596
2400.516381	488439.942041	38.953613
2403.109105	489431.760620	38.958631
2405.531652	490442.830824	38.963648
2408.061264	491447.263615	38.968666
2410.493240	492446.304821	38.973684
2413.187167	493451.300270	38.978701
2415.612900	494443.615711	38.983719
2418.062600	495444.194767	38.988736
2420.407030	496443.168178	38.993754
2422.325925	497441.900526	38.998772
2425.224902	498436.981495	39.003789
2427.914969	499459.328271	39.008807
2430.705436	500453.449601	39.013824
2433.183380	501458.962074	39.018842
2435.514784	502449.155743	39.023860
2438.102636	503436.221661	39.028877
2440.821879	504439.394284	39.033895
2442.831524	505429.662888	39.038912
2445.222856	506418.043452	39.043930
2447.692657	507417.090225	39.048948
2450.346037	508413.876934	39.053965
2452.379288	509424.315806	39.058983
2455.193477	510404.870274	39.064000
2457.600084	511409.980044	39.069018
2459.862862	512399.827842	39.074036
2462.627391	513363.775939	39.079053
2464.742426	514337.398193	39.084071
2467.259120	515290.937373	39.089088
2469.731653	516254.806352	39.094106
2471.753307	517221.662953	39.099124
2474.625041	518184.338554	39.104141
2476.570896	519160.458214	39.109159
2478.893293	520135.647754	39.114176
2481.507688	521109.971419	39.119194
2483.604777	522109.202332	39.124212
2486.215010	523090.149958	39.129229
2488.357278	524088.084617	39.134247
2490.768679	525078.858086	39.139264
2493.667337	526083.334677	39.144282
2496.205560	527096.968104	39.149300
2498.922782	528110.352030	39.154317
2500.838912	529129.387713	39.159335
2503.501739	530145.360325	39.164352
2506.004499	531163.655373	39.169370
2508.579881	532190.526034	39.174388
2510.739959	533223.634631	39.179405
2513.265134	534260.988553	39.184423
2515.773621	535312.211846	39.189440
2518.281546	536349.469289	39.194458
2520.501893	537394.046215	39.199476
2523.149427	538450.854496	39.204493
2525.375294	539528.181837	39.209511
2528.188988	540599.796596	39.214528
2530.816350	541657.627649	39.219546
2533.093976	542733.847482	39.224564
2535.337199	543804.608729	39.229581
2538.055477	544898.546060	39.234599
2540.374261	545985.020566	39.239616
2543.095394	547091.005496	39.244634
2545.753008	548189.018220	39.249652
2548.432701	549282.012562	39.254669
2551.150999	550385.119070	39.259687
2553.634016	551484.254321	39.264704
2556.640459	552591.206740	39.269722
2558.834710	553705.440437	39.274740
2561.037895	554808.473868	39.279757
2563.722027	555911.789821	39.284775
2566.260930	557036.646020	39.289792
2569.180908	558148.733111	39.294810
2571.575841	559275.484064	39.299828
2574.293329	560390.179939	39.304845
2576.858871	561516.008453	39.309863
2579.533237	562644.384638	39.314880
2582.501346	563757.096047	39.319898
2584.964160	564876.675875	39.324916
2587.781300	565996.050543	39.329933
2590.663822	567127.117045	39.334951
2592.913662	568260.196890	39.339968
2595.746761	569364.264799	39.344986
2597.994547	570500.610816	39.350004
2601.288627	571618.011198	39.355021
2603.845279	572738.596711	39.360039
2606.254354	573859.107271	39.365056
2608.883126	574976.069738	39.370074
2611.172969	576102.722658	39.375092
2614.089435	577226.963215	39.380109
2617.122864	578352.337162	39.385127
2619.478265	579473.407017	39.390144
2622.349344	580592.986104	39.395162
2624.935197	581720.584996	39.400180
2627.681336	582836.820791	39.405197
2630.157869	583963.479064	39.410215
2632.776662	585076.271770	39.415232
2635.767615	586157.316730	39.420250
2638.307238	587239.693013	39.425268
2640.636598	588317.896548	39.430285
2643.277988	589394.047273	39.435303
2645.743927	590481.506519	39.440320
2648.481459	591565.965496	39.445338
2651.025146	592643.893739	39.450356
2653.741156	593732.617774	39.455373
2656.145991	594831.462540	39.460391
2658.229488	595935.868084	39.465408
2661.280069	597035.301820	39.470426
2663.820377	598149.240428	39.475444
2666.197957	599260.845768	39.480461
2668.847083	600389.675405	39.485479
2670.843954	601520.004470	39.490496
2673.495484	602657.023489	39.495514
2675.957465	603806.726160	39.500532
2678.539665	604959.647061	39.505549
2681.139937	606130.015444	39.510567
2683.244940	607306.300080	39.515584
2686.341888	608476.344316	39.520602
2688.510199	609676.340003	39.525620
2691.063524	610859.334768	39.530637
2693.946818	612060.608321	39.535655
2696.461254	613276.768351	39.540672
2698.995647	614478.988871	39.545690
2701.713925	615717.702815	39.550708
2704.414029	616938.330593	39.555725
2707.011200	618168.438753	39.560743
2709.435971	619413.883751	39.565760
2712.397702	620657.848441	39.570778
2714.839236	621909.852894	39.575796
2717.732830	623165.485866	39.580813
2720.503841	624431.185934	39.585831
2723.322118	625699.476955	39.590848
2726.369921	626961.285707	39.595866
2728.889575	628237.117656	39.600884
2731.318678	629507.367728	39.605901
2734.706457	630792.288131	39.610919
2737.081102	632076.320366	39.615936
2740.354631	633352.958342	39.620954
2742.961775	634635.690436	39.625972
2745.721572	635923.031161	39.630989
2748.727852	637206.628533	39.636007
2751.361509	638501.704847	39.641024
2754.169703	639776.682596	39.646042
2756.630064	641078.099273	39.651060
2759.225168	642365.860727	39.656077
2762.572998	643661.415141	39.661095
2765.442652	644963.715175	39.666112
2768.318818	646260.960337	39.671130
2771.008407	647549.843514	39.676148
2774.132404	648846.016987	39.681165
2777.161365	650143.882617	39.686183
2779.750776	651441.951036	39.691200
2782.788965	652728.165963	39.696218
2785.583084	654012.809399	39.701236
2788.342762	655303.667891	39.706253
2791.129129	656596.693739	39.711271
2793.727051	657895.008705	39.716288
2796.681145	659188.162655	39.721306
2799.652046	660489.058652	39.726324
2802.207728	661777.851052	39.731341
2805.205594	663070.231552	39.736359
2807.773885	664369.477287	39.741376
2810.993721	665656.745543	39.746394
2813.709264	666955.367672	39.751412
2816.326763	668233.083647	39.756429
2819.561846	669488.838157	39.761447
2822.166286	670748.409559	39.766464
2825.089517	672002.439258	39.771482
2827.798923	673239.630127	39.776500
2830.596688	674498.170380	39.781517
2833.296787	675744.626929	39.786535
2835.920707	677002.907662	39.791552
2838.715329	678260.989707	39.796570
2841.512977	679535.198319	39.801588
2843.799643	680800.372273	39.806605
2846.818854	682075.981251	39.811623
2849.802391	683363.885311	39.816640
2852.310332	684641.853100	39.821658
2855.220932	685935.961061	39.826676
2857.671433	687233.137659	39.831693
2860.761783	688534.589518	39.836711
2863.389698	689847.990437	39.841728
2866.330177	691170.775089	39.846746
2869.070374	692495.878117	39.851764
2871.623862	693818.136022	39.856781
2874.584383	695151.290903	39.861799
2877.195081	696491.593407	39.866816
2880.233583	697849.820827	39.871834
2882.957740	699211.261831	39.876852
2885.906493	700579.245860	39.881869
2889.062006	701944.453739	39.886887
2891.667927	703304.681492	39.891904
2894.760913	704681.908508	39.896922
2897.707469	706057.899892	39.901940
2899.980146	707442.153833	39.906957
2903.313678	708828.337433	39.911975
2906.192613	710224.968171	39.916992
2909.202432	711615.308412	39.922010
2912.065529	713015.543634	39.927028
2914.816178	714424.227161	39.932045
2917.936385	715835.187820	39.937063
2920.896792	717251.825778	39.942080
2923.941078	718654.013065	39.947098
2926.738383	720075.097123	39.952116
2929.426007	721493.434594	39.957133
2932.534935	722929.556117	39.962151
2935.580373	724361.483813	39.967168
2938.459985	725784.639252	39.972186
2941.554206	727216.457014	39.977204
2944.308015	728653.119881	39.982221
2947.577495	730084.504555	39.987239
2950.651510	731519.373508	39.992256
2953.544953	732957.721532	39.997274
2956.850472	734394.658946	40.002292
2959.288776	735843.971655	40.007309
2962.683749	737286.596345	40.012327
2965.563394	738733.486480	40.017344
2968.884768	740182.162188	40.022362
2971.852899	741620.124466	40.027380
2975.081506	743059.705597	40.032397
2978.147255	744500.579036	40.037415
2980.909734	745951.295430	40.042432
2984.357440	747372.793822	40.047450
2987.560408	748813.244546	40.052468
2990.258572	750242.523290	40.057485
2993.282880	751668.824162	40.062503
2996.426580	753110.751427	40.067520
2999.227945	754543.846659	40.072538
3002.764350	755967.246955	40.077556
3005.547068	757408.523871	40.082573
3008.412093	758836.323800	40.087591
3011.574026	760272.368715	40.092608
3014.083059	761685.272101	40.097626
3017.442278	763095.753802	40.102644
3020.464611	764482.910774	40.107661
3023.622329	765863.445297	40.112679
3026.287634	767255.113528	40.117696
3028.755086	768635.986008	40.122714
3031.690028	770034.462681	40.127732
3034.757431	771437.419400	40.132749
3038.126315	772838.045342	40.137767
3040.590593	774245.577340	40.142784
3043.401110	775669.233117	40.147802
3046.849243	777098.201753	40.152820
3049.127493	778529.831752	40.157837
3052.028110	779952.831581	40.162855
3055.084199	781407.715289	40.167872
3058.061488	782863.643085	40.172890
3060.925695	784309.975297	40.177908
3063.654956	785787.471966	40.182925
3066.584122	787264.973249	40.187943
3069.545507	788747.407572	40.192960
3072.556513	790249.372399	40.197978
3075.415575	791760.303877	40.202996
3078.386392	793265.210518	40.208013
3081.829038	794781.912237	40.213031
3084.890996	796301.775759	40.218048
3087.492997	797841.162053	40.223066
3090.661290	799379.282254	40.228084
3093.886760	800919.009057	40.233101
3096.796324	802461.869330	40.238119
3099.921185	804021.320724	40.243136
3103.166733	805598.001946	40.248154
3106.643718	807163.281455	40.253172
3109.331123	808735.663254	40.258189
3112.780656	810307.702061	40.263207
3116.033251	811872.959347	40.268224
3118.761626	813459.382258	40.273242
3122.013668	815049.153470	40.278260
3125.192397	816637.631981	40.283277
3128.167870	818233.087459	40.288295
3131.230020	819827.414223	40.293312
3134.216132	821441.469813	40.298330
3137.940082	823033.012889	40.303348
3140.391379	824652.760365	40.308365
3143.374344	826259.930776	40.313383
3146.905461	827892.690552	40.318400
3149.933809	829507.144719	40.323418
3153.417227	831133.447163	40.328436
3156.427359	832756.253608	40.333453
3160.216493	834388.017857	40.338471
3163.094543	836013.141652	40.343488
3166.067165	837651.220361	40.348506
3169.531130	839279.116455	40.353524
3172.419529	840905.523780	40.358541
3175.782488	842544.273315	40.363559
3179.295476	844178.684300	40.368576
3182.345861	845813.136394	40.373594
3185.735514	847437.583894	40.378612
3188.813096	849086.726247	40.383629
3192.492627	850710.469255	40.388647
3195.721503	852340.173922	40.393664
3198.947458	853972.168511	40.398682
3201.993232	855599.782484	40.403700
3205.415388	857231.173041	40.408717
3208.754299	858860.979458	40.413735
3212.162593	860479.188209	40.418752
3214.979129	862112.382174	40.423770
3218.382747	863738.934291	40.428788
3221.732192	865372.228371	40.433805
3224.932111	866980.694308	40.438823
3227.978074	868572.001737	40.443840
3231.287563	870150.741234	40.448858
3234.693108	871724.014607	40.453876
3237.934818	873294.770529	40.458893
3240.844242	874868.938472	40.463911
3244.161123	876437.688165	40.468928
3246.956980	878020.803150	40.473946
3249.883870	879600.763860	40.478964
3253.015103	881206.453361	40.483981
3256.495233	882805.364564	40.488999
3259.302786	884407.038303	40.494016
3262.375225	886029.951581	40.499034
3265.630252	887640.313633	40.504052
3268.789747	889281.315279	40.509069
3271.848986	890919.742713	40.514087
3274.941930	892563.868755	40.519104
3277.869149	894220.951009	40.524122
3281.382857	895880.153305	40.529140
3284.689703	897548.251631	40.534157
3287.624380	899221.121336	40.539175
3291.036349	900902.757545	40.544192
3293.789704	902604.505568	40.549210
3297.053671	904297.760304	40.554228
3300.123214	906014.876110	40.559245
3303.273443	907730.005862	40.564263
3306.587850	909461.213056	40.569280
3309.766885	911189.304787	40.574298
3313.592828	912926.837732	40.579316
3316.552663	914680.966791	40.584333
3319.942729	916422.842350	40.589351
3323.502622	918182.373966	40.594368
3326.584696	919947.076777	40.599386
3330.123743	921695.202976	40.604404
3333.257778	923473.616484	40.609421
3336.461230	925246.636549	40.614439
3340.052603	927025.044388	40.619456
3343.255849	928816.912736	40.624474
3346.777160	930608.987447	40.629492
3349.989647	932403.762979	40.634509
3353.040266	934196.424312	40.639527
3356.655828	935995.654447	40.644544
3359.988326	937806.079507	40.649562
3363.386580	939604.966805	40.654580
3366.465777	941422.976278	40.659597
3370.116746	943224.585065	40.664615
3373.694138	945041.434892	40.669632
3377.204102	946864.530823	40.674650
3380.250656	948678.847987	40.679668
3383.827773	950503.121890	40.684685
3387.297659	952314.457442	40.689703
3390.666932	954177.415671	40.694720
3393.972841	956051.512437	40.699738
3397.697086	957919.358604	40.704756
3401.276249	959796.104516	40.709773
3404.383825	961674.075513	40.714791
3407.965985	963533.578256	40.719808
3411.405937	965410.958363	40.724826
3414.869446	967276.593176	40.729844
3418.348628	969163.282519	40.734861
3421.614755	971039.631385	40.739879
3424.955667	972911.647963	40.744896
3428.299115	974787.146607	40.749914
3432.042020	976657.774113	40.754932
3435.789359	978533.926381	40.759949
3439.393190	980414.258136	40.764967
3442.963293	982274.504107	40.769984
3445.972325	984136.766089	40.775002
3449.645342	985980.928161	40.780007
3452.837528	987775.816255	40.785012
3456.330995	989516.569852	40.790016
3459.871414	991187.979474	40.795021
3463.141589	992795.224270	40.800026
3466.286667	994314.081451	40.805031
3469.558785	995762.789541	40.810036
3472.408915	997131.465039	40.815040
3475.490562	998414.802164	40.820045
3478.332055	999626.851756	40.825050
3480.982057	1000755.295511	40.830055
3483.755349	1001813.360554	40.835060
3485.781044	1002804.244652	40.840064
3488.806559	1003711.358959	40.845069
3490.628733	1004551.246070	40.850074
3493.080896	1005319.356660	40.855079
3495.015800	1006033.307746	40.860084
3496.713428	1006683.257715	40.865088
3498.962988	1007258.797734	40.870093
3500.323865	1007801.679345	40.875098
3501.980904	1008276.933232	40.880103
3503.535915	1008704.170030	40.885108
3505.229118	1009071.411966	40.890112
3506.406508	1009396.264066	40.895117
3507.680852	1009676.204313	40.900122
3508.913179	1009919.809990	40.905127
3510.216501	1010122.210734	40.910132
3510.964410	1010279.434867	40.915136
3512.214884	1010414.524647	40.920141
3513.175594	1010503.622924	40.925146
3513.959926	1010542.925449	40.930151
3514.957946	1010577.142184	40.935156
3515.812710	1010593.414919	40.940160
3516.741342	1010550.722749	40.945165
3517.105186	1010506.763579	40.950170
3517.542015	1010417.920844	40.955175
3518.392209	1010317.256390	40.960180
3518.904296	1010204.601994	40.965184
3519.790006	1010058.956696	40.970189
3519.945955	1009907.697009	40.975194
3520.473679	1009710.232417	40.980199
3520.838291	1009521.627492	40.985204
3521.262212	1009314.743589	40.990208
3521.758092	1009093.948230	40.995213
3522.050488	1008863.754104	41.000218
3522.493482	1008615.552072	41.005223
3522.825668	1008352.200454	41.010228
3522.869064	1008075.669738	41.015232
3523.391616	1007789.621086	41.020237
3523.571840	1007491.759022	41.025242
3523.928582	1007176.165397	41.030247
3523.820397	1006868.794276	41.035252
3523.883741	1006553.214119	41.040256
3524.689389	1006215.430427	41.045261
3524.567655	1005890.998809	41.050266
3525.007469	1005547.597675	41.055271
3525.207758	1005187.299834	41.060276
3525.395267	1004834.272634	41.065280
3525.539444	1004461.590703	41.070285
3525.673454	1004092.872407	41.075290
3525.654928	1003705.874094	41.080295
3525.855290	1003332.719436	41.085300
3525.419865	1002946.223970	41.090304
3525.667112	1002543.541734	41.095309
3525.582167	1002165.007642	41.100314
3525.586299	1001765.908896	41.105319
3525.623552	1001367.943872	41.110324
3525.679656	1000973.450055	41.115328
3525.993785	1000577.621390	41.120333
3525.939496	1000177.155288	41.125338
3525.925211	999769.356174	41.130343
3526.035341	999364.913177	41.135348
3526.068824	998954.030674	41.140352
3526.147092	998538.049867	41.145357
3526.401694	998131.743028	41.150362
3526.451457	997697.503338	41.155367
3526.366332	997271.527371	41.160372
3526.151078	996838.433668	41.165376
3526.243790	996416.258401	41.170381
3526.241135	995997.378052	41.175386
3526.248906	995560.741898	41.180391
3526.472643	995144.000925	41.185396
3525.977621	994717.413500	41.190400
3526.282236	994280.435048	41.195405
3526.074946	993861.430572	41.200410
3526.191271	993417.208359	41.205415
3526.265962	992983.772324	41.210420
3525.617493	992553.052967	41.215424
3526.086491	992122.604020	41.220429
3526.103295	991698.433502	41.225434
3525.747480	991250.513965	41.230439
3525.707194	990819.367952	41.235444
3525.555007	990399.903888	41.240448
3525.717311	989959.887098	41.245453
3525.739213	989525.708387	41.250458
3525.316351	989110.093036	41.255463
3525.416273	988677.981515	41.260468
3525.357512	988249.666012	41.265472
3525.437964	987814.371906	41.270477
3525.395666	987386.281213	41.275482
3525.591313	986953.925425	41.280487
3525.693017	986512.579036	41.285492
3525.388287	986094.480511	41.290496
3525.598810	985652.659357	41.295501
3525.459380	985222.373349	41.300506
3525.081919	984782.435128	41.305511
3525.467504	984350.240578	41.310516
3524.940318	983921.774062	41.315520
3525.234020	983489.236612	41.320525
3525.088614	983057.226652	41.325530
3525.134014	982627.982970	41.330535
3525.169934	982195.780264	41.335540
3524.573525	981766.967931	41.340544
3524.897159	981337.776539	41.345549
3524.614601	980908.652728	41.350554
3524.939936	980478.517754	41.355559
3524.811468	980045.691044	41.360564
3524.477091	979623.509637	41.365568
3524.460088	979196.654685	41.370573
3524.154851	978772.159336	41.375578
3524.283353	978351.663327	41.380583
3524.222829	977930.288374	41.385588
3524.073748	977518.568166	41.390592
3523.974892	977089.908563	41.395597
3524.051353	976677.015921	41.400602
3523.794587	976260.142226	41.405607
3523.929522	975843.955350	41.410612
3523.700513	975414.116656	41.415616
3524.019540	974993.537684	41.420621
3523.607744	974584.092745	41.425626
3523.505040	974163.229010	41.430631
3523.639159	973740.437998	41.435636
3523.610245	973325.756772	41.440640
3523.514978	972902.452873	41.445645
3523.587535	972496.787322	41.450650
3523.339732	972076.478531	41.455655
3523.372713	971666.067140	41.460660
3523.322627	971261.898988	41.465664
3523.321612	970842.534789	41.470669
3522.819779	970442.393198	41.475674
3522.975603	970028.225335	41.480679
3522.983858	969621.290852	41.485684
3523.058903	969216.762270	41.490688
3523.150110	968816.507364	41.495693
3522.887182	968400.823431	41.500698
3522.565897	967998.720389	41.505703
3522.749040	967583.686603	41.510708
3522.375769	967186.819618	41.515712
3522.969634	966783.502051	41.520717
3522.438703	966381.711780	41.525722
3522.082118	965981.137193	41.530727
3522.214101	965585.446718	41.535732
3522.057045	965176.364374	41.540736
3522.562479	964782.515102	41.545741
3522.066801	964395.951431	41.550746
3522.116596	963992.429712	41.555751
3521.977643	963599.388926	41.560756
3521.505204	963202.458886	41.565760
3521.655112	962807.063908	41.570765
3521.500502	962433.827855	41.575770
3521.555919	962041.726038	41.580775
3521.580162	961649.798569	41.585780
3521.506211	961266.775531	41.590784
3521.644021	960873.698900	41.595789
3521.476548	960488.582078	41.600794
3521.181669	960103.362508	41.605799
3521.405736	959723.715253	41.610804
3521.297509	959342.627746	41.615808
3521.345714	958957.863066	41.620813
3520.804648	958578.658452	41.625818
3520.671924	958194.166638	41.630823
3520.885310	957809.788217	41.635828
3520.548666	957442.434228	41.640832
3520.647174	957063.808865	41.645837
3520.729585	956701.730743	41.650842
3520.505635	956323.109897	41.655847
3520.635514	955949.897093	41.660852
3520.332990	955589.675692	41.665856
3520.373122	955208.977000	41.670861
3520.284725	954847.202958	41.675866
3520.297556	954477.150724	41.680871
3520.385320	954107.945231	41.685876
3520.167283	953747.496896	41.690880
3519.790548	953376.849792	41.695885
3519.923570	953010.313514	41.700890
3519.896873	952648.195380	41.705895
3519.825800	952297.104128	41.710900
3519.888667	951946.996503	41.715904
3519.490228	951589.959173	41.720909
3519.673366	951247.817344	41.725914
3519.212800	950902.889055	41.730919
3519.240523	950557.665685	41.735924
3518.944017	950216.777297	41.740928
3519.464486	949876.592611	41.745933
3519.102797	949545.906998	41.750938
3519.046760	949204.720156	41.755943
3519.039504	948860.536149	41.760948
3518.756902	948522.116158	41.765952
3519.084353	948187.784232	41.770957
3519.238913	947840.251177	41.775962
3518.881329	947510.869159	41.780967
3518.899976	947168.290197	41.785972
3518.671685	946841.045521	41.790976
3518.572340	946500.451771	41.795981
3518.610931	946178.960775	41.800986
3518.720450	945841.831414	41.805991
3518.622733	945500.405273	41.810996
3518.526370	945176.863178	41.816000
3518.641428	944829.707824	41.821005
3518.419041	944498.099666	41.826010
3517.941022	944165.267223	41.831015
3518.189068	943837.849165	41.836020
3517.683182	943524.040881	41.841024
3518.045743	943192.060999	41.846029
3518.090497	942880.517871	41.851034
3517.899942	942561.138609	41.856039
3517.771531	942239.429920	41.861044
3517.431516	941927.892931	41.866048
3517.640534	941605.035317	41.871053
3517.426848	941289.989549	41.876058
3517.339873	940984.583260	41.881063
3517.493962	940666.851565	41.886068
3517.037645	940359.648429	41.891072
3517.036580	940040.082929	41.896077
3516.956440	939739.682690	41.901082
3516.984352	939433.399597	41.906087
3516.714485	939132.899788	41.911092
3516.834907	938827.620465	41.916096
3516.635710	938534.744632	41.921101
3516.614864	938238.946400	41.926106
3516.813350	937933.026629	41.931111
3516.979247	937623.546119	41.936116
3516.782521	937331.177850	41.941120
3516.700516	937028.703946	41.946125
3516.498438	936730.068931	41.951130
3516.615103	936421.005057	41.956135
3516.763696	936126.306523	41.961140
3516.646500	935830.100343	41.966144
3516.480050	935524.867570	41.971149
3516.504775	935237.142891	41.976154
3516.336753	934934.946243	41.981159
3516.361777	934633.372099	41.986164
3515.933714	934352.006460	41.991168
3516.065837	934055.467322	41.996173
3515.965111	933769.602344	42.001178
3515.888299	933484.101821	42.006183
3516.008316	933190.875124	42.011188
3515.659101	932912.586955	42.016192
3516.057311	932628.209671	42.021197
3515.755851	932337.692731	42.026202
3515.541935	932047.529398	42.031207
3515.436605	931766.356701	42.036212
3515.341261	931490.639972	42.041216
3515.438363	931200.763014	42.046221
3515.150359	930935.610759	42.051226
3514.742799	930650.971927	42.056231
3515.164534	930390.092609	42.061236
3514.742908	930125.786141	42.066240
3514.890991	929841.012322	42.071245
3514.750379	929584.219716	42.076250
3514.886038	929309.119891	42.081255
3515.016572	929043.419972	42.086260
3514.694374	928776.820785	42.091264
3514.643378	928504.495812	42.096269
3514.585241	928250.507150	42.101274
3514.356007	927983.564727	42.106279
3514.887128	927723.593427	42.111284
3514.571358	927460.001770	42.116288
3514.473465	927190.115525	42.121293
3514.433197	926938.463624	42.126298
3514.040011	926670.617701	42.131303
3514.289665	926415.914431	42.136308
3513.750595	926156.715891	42.141312
3513.996610	925906.217612	42.146317
3513.885931	925653.747964	42.151322
3513.993226	925402.672295	42.156327
3514.282415	925149.824666	42.161332
3513.633019	924903.560346	42.166336
3513.689756	924643.805905	42.171341
3513.601534	924398.483405	42.176346
3513.570565	924150.063722	42.181351
3513.534707	923899.902722	42.186356
3513.111804	923667.293258	42.191360
3513.262535	923426.213760	42.196365
3513.357639	923190.998327	42.201370
3513.259057	922949.938563	42.206375
3513.574176	922698.317568	42.211380
3513.416585	922464.650719	42.216384
3513.455022	922219.881172	42.221389
3512.963691	921976.919041	42.226394
3512.914824	921743.203005	42.231399
3513.037193	921504.254428	42.236404
3513.078845	921277.813697	42.241408
3513.248625	921039.894889	42.246413
3512.739406	920813.910255	42.251418
3512.692082	920583.414621	42.256423
3513.089521	920351.488958	42.261428
3512.607732	920118.255001	42.266432
3512.794270	919877.492101	42.271437
3512.737827	919643.494088	42.276442
3512.578799	919416.912295	42.281447
3512.795131	919178.711548	42.286452
3512.459913	918959.645640	42.291456
3512.343114	918733.124551	42.296461
3512.486412	918510.497093	42.301466
3512.658278	918283.139736	42.306471
3512.552421	918057.358626	42.311476
3512.159491	917832.289208	42.316480
3512.347210	917615.874310	42.321485
3512.248581	917399.401716	42.326490
3512.218754	917186.182212	42.331495
3512.198008	916958.223606	42.336500
3512.212607	916736.507429	42.341504
3512.412065	916519.950766	42.346509
3512.094636	916299.426839	42.351514
3511.892014	916080.415642	42.356519
3512.299151	915850.125644	42.361524
3511.524148	915644.575449	42.366528
3511.547488	915431.182253	42.371533
3511.521055	915223.278046	42.376538
3511.647618	915014.570292	42.381543
3511.693718	914803.941674	42.386548
3511.280814	914605.226864	42.391552
3511.425960	914383.393616	42.396557
3511.650282	914183.402726	42.401562
3511.331628	913977.810974	42.406567
3511.612156	913773.365027	42.411572
3511.412548	913570.050182	42.416576
3511.544918	913358.099455	42.421581
3511.093618	913162.999296	42.426586
3511.312402	912953.427114	42.431591
3511.325512	912746.385761	42.436596
3510.786876	912554.554049	42.441600
3510.882577	912353.072403	42.446605
3510.852131	912156.807287	42.451610
3510.732211	911960.838979	42.456615
3510.806563	911765.891654	42.461620
3510.853444	911569.111022	42.466624
3511.117197	911377.009658	42.471629
3510.833200	911185.570062	42.476634
3510.792293	910980.976796	42.481639
3510.797471	910788.897524	42.486644
3510.713713	910600.874237	42.491648
3510.712556	910408.589997	42.496653
3510.678526	910213.509212	42.501658
3510.543923	910025.089122	42.506663
3510.428496	909834.731543	42.511668
3510.629438	909655.786658	42.516672
3510.468740	909460.507339	42.521677
3510.844073	909277.086997	42.526682
3510.233323	909087.363699	42.531687
3510.369265	908889.605146	42.536692
3510.152332	908713.205295	42.541696
3510.117897	908524.621133	42.546701
3510.160658	908344.213611	42.551706
3509.968047	908166.249589	42.556711
3510.187430	907988.115549	42.561716
3509.866982	907812.379045	42.566720
3509.837747	907633.888862	42.571725
3509.712820	907451.069063	42.576730
3509.916714	907273.203924	42.581735
3509.962313	907105.485628	42.586740
3509.580667	906938.507772	42.591744
3509.637077	906746.569029	42.596749
3509.647311	906576.236464	42.601754
3509.896693	906413.093369	42.606759
3509.913593	906228.087948	42.611764
3509.630323	906070.520639	42.616768
3509.506829	905887.166834	42.621773
3509.589259	905724.416904	42.626778
3509.410132	905555.434807	42.631783
3509.818556	905381.334227	42.636788
3509.327804	905220.882875	42.641792
3509.528328	905044.201187	42.646797
3509.368132	904879.536985	42.651802
3509.325799	904712.725858	42.656807
3509.500996	904546.645799	42.661812
3509.632352	904376.418967	42.666816
3509.881157	904211.860658	42.671821
3509.802344	904038.570390	42.676826
3509.576584	903863.465482	42.681831
3509.817990	903685.286570	42.686836
3509.421856	903526.218410	42.691840
3509.422104	903357.622712	42.696845
3509.683565	903197.085750	42.701850
3509.466029	903027.164832	42.706855
3509.531250	902850.629083	42.711860
3509.097124	902688.358322	42.716864
3509.324457	902519.410407	42.721869
3508.943107	902354.611712	42.726874
3508.870255	902190.915673	42.731879
3509.538457	902032.594988	42.736884
3509.186608	901881.581315	42.741888
3509.103320	901706.578518	42.746893
3509.149046	901550.760186	42.751898
3509.009444	901382.996952	42.756903
3509.214908	901217.778550	42.761908
3508.975588	901054.076770	42.766912
3508.970111	900898.731518	42.771917
3508.902158	900747.544012	42.776922
3508.364779	900596.333222	42.781927
3508.882333	900434.612912	42.786932
3508.385264	900283.097383	42.791937
3508.824933	900132.871887	42.796941
3508.719906	899984.277168	42.801946
3508.567841	899839.645558	42.806951
3508.571751	899675.960159	42.811956
3508.537242	899530.625252	42.816961
3508.575419	899379.383509	42.821965
3508.824742	899220.569812	42.826970
3508.436247	899069.872951	42.831975
3508.587378	898910.197464	42.836980
3508.500085	898764.465172	42.841985
3508.177478	898613.262325	42.846989
3508.039198	898466.371669	42.851994
3508.110079	898331.903323	42.856999
3508.403635	898186.769531	42.862004
3508.095839	898051.680729	42.867009
3508.159667	897900.781535	42.872013
3508.081905	897755.311437	42.877018
3508.166914	897610.873446	42.882023
3508.026750	897463.570612	42.887028
3507.621869	897325.292366	42.892033
3507.792273	897184.114180	42.897037
3508.079419	897052.284950	42.902042
3507.667664	896922.790003	42.907047
3507.437323	896784.373169	42.912052
3507.482470	896641.849424	42.917057
3507.831985	896507.001938	42.922061
3508.210017	896372.726312	42.927066
3507.649044	896248.458392	42.932071
3507.475324	896105.280815	42.937076
3507.494649	895974.436964	42.942081
3507.716140	895842.107249	42.947085
3507.718086	895701.982910	42.952090
3507.412043	895581.233993	42.957095
3507.759052	895448.874439	42.962100
3507.623254	895321.423594	42.967105
3507.656315	895177.608685	42.972109
3507.890795	895042.262135	42.977114
3507.250571	894925.033712	42.982119
3507.462911	894794.807456	42.987124
3507.446558	894660.846308	42.992129
3507.364913	894536.945233	42.997133
3507.353420	894410.323412	43.002138
3507.295435	894283.899758	43.007143
3507.481722	894145.446617	43.012148
3507.138399	894020.417432	43.017153
3507.239364	893882.841968	43.022157
3507.069482	893760.968603	43.027162
3507.156069	893644.850785	43.032167
3507.126556	893520.048940	43.037172
3507.313671	893402.556171	43.042177
3507.311032	893270.686979	43.047181
3507.173147	893156.529798	43.052186
3506.857957	893033.311276	43.057191
3507.271509	892907.939629	43.062196
3507.075350	892797.458930	43.067201
3506.982968	892675.452916	43.072205
3506.984583	892545.306685	43.077210
3506.797507	892429.886082	43.082215
3506.877834	892303.975921	43.087220
3506.641401	892188.848669	43.092225
3506.602464	892068.851558	43.097229
3506.618833	891962.090993	43.102234
3506.530417	891850.413809	43.107239
3506.531461	891732.240421	43.112244
3506.334998	891631.697923	43.117249
3506.402454	891519.408354	43.122253
3506.791912	891405.709576	43.127258
3506.556917	891295.593096	43.132263
3506.711807	891173.997881	43.137268
3506.392091	891069.403774	43.142273
3506.488780	890957.581962	43.147277
3506.553722	890862.495866	43.152282
3506.356528	890748.687266	43.157287
3506.504415	890631.821101	43.162292
3506.609110	890529.758781	43.167297
3506.568355	890416.111260	43.172301
3506.604534	890303.512843	43.177306
3506.375899	890201.402869	43.182311
3506.378037	890082.227966	43.187316
3505.966865	889988.463361	43.192321
3506.453854	889874.331228	43.197325
3506.441672	889764.438847	43.202330
3506.011821	889669.898204	43.207335
3506.458136	889554.992510	43.212340
3506.034583	889460.060406	43.217345
3506.051086	889347.543235	43.222349
3505.882926	889244.632318	43.227354
3506.257329	889147.531888	43.232359
3506.036626	889050.721364	43.237364
3506.081248	888957.348593	43.242369
3506.097735	888849.756067	43.247373
3505.770290	888752.958118	43.252378
3506.040684	888660.220624	43.257383
3505.904965	888547.035576	43.262388
3506.089310	888458.566426	43.267393
3506.241182	888345.136510	43.272397
3506.208689	888253.603527	43.277402
3506.003787	888154.743279	43.282407
3505.991533	888054.107778	43.287412
3505.756788	887960.281030	43.292417
3505.776993	887847.056544	43.297421
3505.813966	887745.343060	43.302426
3505.857158	887662.304229	43.307431
3505.997907	887553.312187	43.312436
3505.763598	887456.864220	43.317441
3505.694750	887367.161933	43.322445
3505.851088	887278.001837	43.327450
3505.564150	887184.848539	43.332455
3505.829966	887086.957044	43.337460
3505.859330	887000.039608	43.342465
3505.597912	886899.908955	43.347469
3505.838957	886810.146962	43.352474
3505.622892	886725.588757	43.357479
3505.843954	886615.791475	43.362484
3505.497792	886520.894972	43.367489
3505.371073	886433.607558	43.372493
3505.340541	886344.657442	43.377498
3505.224447	886261.527923	43.382503
3505.338904	886181.263200	43.387508
3505.395577	886088.906816	43.392513
3505.682242	885999.608736	43.397517
3505.814969	885901.138289	43.402522
3505.304149	885809.064541	43.407527
3505.476284	885722.104380	43.412532
3505.272132	885634.527249	43.417537
3505.519466	885550.262751	43.422541
3505.708544	885467.361981	43.427546
3505.279675	885377.881770	43.432551
3505.602942	885293.891474	43.437556
3505.442636	885200.975797	43.442561
3505.281004	885114.642403	43.447565
3505.419393	885027.193294	43.452570
3505.425305	884938.893313	43.457575
3505.384781	884852.342423	43.462580
3505.697703	884765.732012	43.467585
3505.403836	884681.447233	43.472589
3505.628681	884583.229699	43.477594
3505.317691	884506.594435	43.482599
3505.490255	884415.063735	43.487604
3505.311841	884337.823428	43.492609
3505.306835	884245.157347	43.497613
3505.549645	884157.290606	43.502618
3505.265209	884075.706798	43.507623
3505.319886	883971.019051	43.512628
3505.125138	883883.898118	43.517633
3505.310147	883808.140293	43.522637
3505.438430	883719.995297	43.527642
3505.392459	883649.212304	43.532647
3505.356743	883555.378189	43.537652
3505.118652	883476.102557	43.542657
3505.088165	883394.273656	43.547661
3505.310518	883314.532582	43.552666
3505.096409	883227.017608	43.557671
3505.251740	883141.667999	43.562676
3504.985291	883067.137104	43.567681
3504.786605	882987.945179	43.572685
3504.923814	882906.856617	43.577690
3504.883300	882827.152177	43.582695
3505.091722	882746.630784	43.587700
3504.791857	882678.299220	43.592705
3505.070572	882596.795602	43.597709
3504.881435	882516.530245	43.602714
3504.569384	882450.328939	43.607719
3504.749605	882373.003454	43.612724
3504.908325	882298.198946	43.617729
3504.941244	882210.143676	43.622733
3505.099536	882132.721754	43.627738
3504.626428	882061.602369	43.632743
3504.898484	881985.612769	43.637748
3504.771083	881906.878753	43.642753
3504.710120	881836.269940	43.647757
3505.095821	881762.874250	43.652762
3504.665844	881694.358841	43.657767
3504.924378	881609.454174	43.662772
3504.818436	881539.042927	43.667777
3504.720081	881456.810502	43.672781
3504.929604	881397.486512	43.677786
3504.699307	881316.533274	43.682791
3504.731116	881231.466708	43.687796
3504.797673	881166.932327	43.692801
3504.717725	881094.380021	43.697805
3504.430021	881015.466627	43.702810
3504.465304	880949.966152	43.707815
3504.673857	880887.536789	43.712820
3504.491620	880810.540998	43.717825
3504.655542	880740.269443	43.722829
3504.727133	880662.551657	43.727834
3504.330538	880603.900822	43.732839
3504.439713	880519.876971	43.737844
3504.477490	880455.823953	43.742849
3504.526208	880392.834281	43.747853
3504.509288	880324.428541	43.752858
3504.542792	880262.602734	43.757863
3504.760414	880189.699490	43.762868
3504.540994	880116.770441	43.767873
3504.453186	880047.307243	43.772877
3504.613910	879978.286787	43.777882
3504.331347	879919.028884	43.782887
3504.684563	879845.517600	43.787892
3504.631980	879785.735937	43.792897
3504.505553	879713.367977	43.797901
3504.697010	879636.004450	43.802906
3504.415193	879566.470606	43.807911
3504.799371	879489.170301	43.812916
3504.217795	879422.979092	43.817921
3504.388675	879353.271226	43.822925
3504.396188	879292.602420	43.827930
3504.542200	879230.844108	43.832935
3504.403223	879157.889873	43.837940
3504.427636	879107.877105	43.842945
3504.268822	879034.924609	43.847949
3504.436805	878975.486020	43.852954
3504.252644	878909.901973	43.857959
3504.195377	878842.842471	43.862964
3504.315906	878781.471316	43.867969
3504.276193	878717.218227	43.872973
3504.430260	878644.887798	43.877978
3504.263754	878586.857325	43.882983
3504.495597	878513.640140	43.887988
3504.470187	878452.871155	43.892993
3504.202738	878385.744135	43.897997
3504.387228	878315.343211	43.903002
3504.012671	878248.135335	43.908007
3504.382510	878184.390531	43.913012
3504.295024	878130.122871	43.918017
3504.407458	878069.908815	43.923021
3504.149719	878000.158578	43.928026
3503.910072	877945.138798	43.933031
3504.222894	877875.002269	43.938036
3504.180045	877823.341722	43.943041
3503.869557	877761.643182	43.948045
3503.907467	877704.248888	43.953050
3503.962387	877649.177810	43.958055
3504.172434	877575.661722	43.963060
3504.274431	877509.045477	43.968065
3503.906670	877458.986349	43.973069
3503.936082	877395.192145	43.978074
3503.565576	877344.066097	43.983079
3503.712237	877283.935308	43.988084
3503.707560	877232.263285	43.993089
3503.783576	877183.776811	43.998093
3503.574634	877139.408750	44.003098
3503.667700	877077.830451	44.008103
3503.841663	877023.703415	44.013108
3503.666496	876980.104197	44.018113
3503.813341	876930.149692	44.023117
3503.810345	876869.069803	44.028122
3503.565428	876814.525089	44.033127
3503.786500	876765.138684	44.038132
3503.550583	876711.658043	44.043137
3503.809758	876664.979295	44.048141
3503.752767	876609.916942	44.053146
3503.700467	876553.301963	44.058151
3503.999335	876493.525874	44.063156
3503.507296	876447.841809	44.068161
3503.419844	876387.643492	44.073165
3503.783678	876339.199619	44.078170
3503.505897	876287.079495	44.083175
3503.582703	876236.742807	44.088180
3503.815299	876191.131296	44.093185
3503.616426	876145.881414	44.098189
3503.695796	876082.840506	44.103194
3503.501473	876040.498060	44.108199
3503.683869	875991.887298	44.113204
3503.672498	875940.883840	44.118209
3503.718055	875883.664503	44.123213
3503.758916	875833.233329	44.128218
3503.474043	875784.019046	44.133223
3503.571459	875738.717229	44.138228
3503.374617	875687.451223	44.143233
3503.547241	875644.172723	44.148237
3503.696693	875583.733232	44.153242
3503.726322	875530.392084	44.158247
3503.710927	875480.258094	44.163252
3503.480485	875437.432391	44.168257
3503.753765	875387.347031	44.173261
3503.824404	875336.227866	44.178266
3503.547398	875295.348379	44.183271
3503.675552	875235.490716	44.188276
3503.762593	875192.513954	44.193281
3503.308735	875131.781316	44.198285
3503.437860	875087.439108	44.203290
3503.625864	875047.645091	44.208295
3503.445988	874985.702013	44.213300
3503.765865	874947.340363	44.218305
3503.612203	874896.642295	44.223309
3503.566440	874838.942964	44.228314
3502.887956	874796.768356	44.233319
3503.364914	874763.132023	44.238324
3503.474374	874715.589661	44.243329
3503.345754	874674.972405	44.248333
3503.508389	874627.226594	44.253338
3503.172276	874582.472300	44.258343
3503.679837	874533.505015	44.263348
3503.671095	874481.130650	44.268353
3503.161022	874435.336983	44.273357
3503.444695	874375.057027	44.278362
3503.203285	874344.931482	44.283367
3503.316547	874298.161104	44.288372
3503.479345	874261.275831	44.293377
3503.199408	874219.613420	44.298381
3503.310342	874176.043363	44.303386
3503.333580	874135.979377	44.308391
3503.661686	874086.455979	44.313396
3503.456862	874039.444968	44.318401
3502.922112	873988.898911	44.323405
3503.007192	873948.241464	44.328410
3503.359498	873909.091745	44.333415
3503.401856	873858.352494	44.338420
3503.263367	873824.521232	44.343425
3503.383377	873786.476015	44.348429
3503.402176	873740.395831	44.353434
3503.583636	873701.369896	44.358439
3503.103452	873645.573620	44.363444
3503.214267	873609.371904	44.368449
3503.110593	873564.280599	44.373453
3503.359180	873525.145439	44.378458
3503.136956	873484.244416	44.383463
3503.064153	873437.788938	44.388468
3503.432188	873402.901723	44.393473
3503.045846	873359.116564	44.398477
3503.212661	873319.411454	44.403482
3502.879380	873277.557185	44.408487
3502.929238	873228.848577	44.413492
3503.194554	873192.133798	44.418497
3503.293350	873167.281973	44.423501
3503.240757	873118.298295	44.428506
3503.100825	873074.567454	44.433511
3503.248193	873035.251713	44.438516
3503.170873	872993.353269	44.443521
3503.045287	872953.693890	44.448525
3503.313877	872912.999121	44.453530
3503.089569	872879.176608	44.458535
3503.211718	872828.415410	44.463540
3503.227127	872793.679739	44.468545
3502.941056	872752.493131	44.473549
3503.225713	872702.480253	44.478554
3503.132991	872669.216996	44.483559
3502.914949	872633.742672	44.488564
3503.304438	872588.562710	44.493569
3503.090900	872542.996633	44.498573
3503.056138	872509.140785	44.503578
3502.836540	872473.083609	44.508583
3503.008425	872436.476585	44.513588
3503.493267	872410.490710	44.518593
3503.037662	872368.747213	44.523597
3502.861913	872330.935459	44.528602
3502.741188	872295.346054	44.533607
3502.981722	872260.570180	44.538612
3503.036650	872221.167260	44.543617
3503.082363	872190.498318	44.548621
3502.932308	872147.732626	44.553626
3502.805757	872104.962754	44.558631
3502.693684	872073.251856	44.563636
3503.006670	872044.672835	44.568641
3502.916288	872012.763975	44.573645
3503.178818	871968.182425	44.578650
3503.132215	871933.646016	44.583655
3502.864809	871900.116134	44.588660
3502.864140	871862.951805	44.593665
3502.739446	871823.575846	44.598669
3503.125979	871790.713900	44.603674
3502.497461	871755.496035	44.608679
3502.737650	871727.121560	44.613684
3503.155002	871694.933273	44.618689
3502.774656	871659.382837	44.623693
3503.152852	871621.184194	44.628698
3502.965447	871587.639370	44.633703
3503.015986	871552.599548	44.638708
3503.033061	871508.152037	44.643713
3502.838422	871479.362816	44.648717
3503.048913	871440.123184	44.653722
3502.839866	871410.947836	44.658727
3503.166328	871372.076822	44.663732
3503.018671	871349.198881	44.668737
3502.624873	871307.243659	44.673741
3502.844098	871274.697570	44.678746
3502.675046	871237.848219	44.683751
3502.964816	871200.340771	44.688756
3502.683762	871173.117046	44.693761
3502.474664	871142.387643	44.698765
3502.910574	871102.332274	44.703770
3502.599642	871089.670255	44.708775
3502.812615	871047.322091	44.713780
3502.647690	871021.534273	44.718785
3502.620172	870986.503984	44.723789
3502.930192	870955.882194	44.728794
3502.744913	870923.691985	44.733799
3502.619835	870900.905654	44.738804
3502.948951	870852.131592	44.743809
3502.943855	870833.110259	44.748813
3503.087103	870788.927758	44.753818
3502.535543	870765.822961	44.758823
3502.787705	870724.533639	44.763828
3502.786236	870696.097025	44.768833
3502.829156	870662.800212	44.773837
3502.737235	870628.651928	44.778842
3502.373600	870598.818683	44.783847
3502.813681	870576.617395	44.788852
3502.786377	870547.796104	44.793857
3502.624505	870517.055697	44.798861
3502.671465	870484.824858	44.803866
3502.622509	870465.615464	44.808871
3502.529004	870433.213371	44.813876
3502.561551	870413.019793	44.818881
3502.524085	870373.134587	44.823885
3503.059695	870344.704875	44.828890
3502.738092	870315.542709	44.833895
3502.767174	870286.225563	44.838900
3502.978941	870250.277981	44.843905
3502.619035	870213.162558	44.848909
3502.826041	870177.894762	44.853914
3502.415885	870149.619940	44.858919
3502.498352	870122.719780	44.863924
3502.532788	870104.563188	44.868929
3502.701582	870072.310051	44.873933
3502.710780	870042.412598	44.878938
3502.455797	870011.296666	44.883943
3502.669161	869988.936421	44.888948
3502.594976	869952.742964	44.893953
3502.503932	869933.927061	44.898957
3502.816992	869889.224598	44.903962
3502.471861	869865.985230	44.908967
3502.527612	869835.787870	44.913972
3502.874870	869804.280434	44.918977
3502.830985	869785.553363	44.923981
3502.784091	869757.993391	44.928986
3502.543103	869730.174059	44.933991
3502.763493	869679.855226	44.938996
3502.521172	869656.015677	44.944001
3502.781858	869628.598577	44.949005
3503.013868	869594.973448	44.954010
3502.768115	869570.454617	44.959015
3502.609992	869531.748548	44.964020
3502.623250	869509.419481	44.969025
3502.492270	869476.630080	44.974029
3502.842623	869446.964668	44.979034
3503.014168	869426.550709	44.984039
3502.943083	869382.393126	44.989044
3502.791485	869352.421640	44.994049
3502.484185	869330.338870	44.999053
3502.545805	869293.536589	45.004058
3502.387639	869282.010483	45.009063
3502.519636	869244.419686	45.014068
3502.670217	869219.834120	45.019073
3502.449366	869187.640412	45.024077
3502.485271	869162.685188	45.029082
3502.645581	869145.572821	45.034087
3502.557464	869105.007944	45.039092
3502.636493	869089.850416	45.044097
3502.762466	869057.793031	45.049101
3502.696025	869021.301419	45.054106
3502.326333	868997.383146	45.059111
3502.286055	868968.944710	45.064116
3502.332362	868938.356049	45.069121
3502.245609	868915.652913	45.074125
3502.423215	868895.527398	45.079130
3502.496419	868869.593970	45.084135
3502.378564	868852.526596	45.089140
3502.690823	868827.330277	45.094145
3502.012352	868797.248642	45.099149
3502.426099	868780.967250	45.104154
3502.449905	868752.128885	45.109159
3502.425422	868721.647866	45.114164
3502.436149	868711.646219	45.119169
3502.462921	868677.661410	45.124173
3502.556905	868660.752763	45.129178
3502.498702	868634.645794	45.134183
3502.568807	868609.488456	45.139188
3502.763884	868579.553072	45.144193
3502.862238	868565.167745	45.149197
3502.841681	868520.898396	45.154202
3502.575354	868502.398138	45.159207
3502.274361	868463.902882	45.164212
3502.654111	868431.509067	45.169217
3502.618862	868417.339579	45.174221
3502.925418	868369.422835	45.179226
3502.529073	868355.506876	45.184231
3502.547086	868317.152306	45.189236
3502.820208	868302.252090	45.194241
3502.940339	868273.492647	45.199245
3502.946300	868231.838328	45.204250
3502.667658	868202.270392	45.209255
3502.930403	868165.525147	45.214260
3502.645527	868142.463340	45.219265
3502.622590	868114.212185	45.224269
3502.987079	868082.401581	45.229274
3502.923615	868052.506165	45.234279
3502.661572	868021.963631	45.239284
3502.895748	867978.522193	45.244289
3502.647821	867957.298458	45.249293
3502.803403	867914.354999	45.254298
3502.621944	867894.673685	45.259303
3502.855002	867862.398071	45.264308
3502.764300	867831.632138	45.269313
3502.705669	867805.521631	45.274317
3503.048659	867773.615834	45.279322
3502.522318	867750.203892	45.284327
3502.546687	867717.573473	45.289332
3502.478615	867695.639461	45.294337
3502.655261	867666.188077	45.299341
3502.631538	867625.408373	45.304346
3502.140978	867620.634018	45.309351
3502.641571	867584.817080	45.314356
3502.957608	867560.100352	45.319361
3502.392810	867534.848901	45.324365
3502.550761	867505.302704	45.329370
3502.603297	867484.222005	45.334375
3502.654096	867446.827539	45.339380
3502.617489	867414.788164	45.344385
3502.413927	867398.216307	45.349389
3502.526595	867365.083887	45.354394
3502.322672	867345.792907	45.359399
3502.489732	867321.391069	45.364404
3502.501555	867292.741885	45.369409
3502.274314	867268.599014	45.374413
3502.434621	867250.510151	45.379418
3502.194221	867225.398170	45.384423
3502.236315	867206.745986	45.389428
3502.408505	867196.132547	45.394433
3502.266368	867167.508131	45.399437
3502.644496	867148.023509	45.404442
3502.410117	867123.589896	45.409447
3502.718281	867091.200658	45.414452
3502.735019	867069.153272	45.419457
3502.214562	867048.262559	45.424461
3502.505464	867024.713138	45.429466
3502.429516	867001.321178	45.434471
3502.478102	866964.992338	45.439476
3502.649446	866939.325751	45.444481
3502.175094	866918.815453	45.449485
3502.601973	866891.455596	45.454490
3502.415907	866865.361997	45.459495
3502.397998	866844.193544	45.464500
3502.589775	866813.375857	45.469505
3502.362781	866797.680259	45.474509
3502.642908	866753.542579	45.479514
3502.000185	866738.886502	45.484519
3502.022092	866726.645979	45.489524
3502.156891	866708.656809	45.494529
3502.296235	866686.393583	45.499533
3502.351833	866664.921031	45.504538
3502.505071	866651.007680	45.509543
3502.533349	866625.848929	45.514548
3502.533798	866605.939178	45.519553
3502.341603	866571.492925	45.524557
3502.940374	866549.930474	45.529562
3502.906603	866519.148442	45.534567
3502.408066	866496.406873	45.539572
3502.738419	866460.125687	45.544577
3502.438915	866449.103029	45.549581
3502.682498	866412.641606	45.554586
3502.379946	866393.169567	45.559591
3502.538914	866367.308335	45.564596
3502.812504	866329.481721	45.569601
3502.321434	866303.921561	45.574605
3502.229269	866272.759387	45.579610
3502.682635	866261.126717	45.584615
3502.419895	866228.049888	45.589620
3502.585728	866203.546597	45.594625
3502.646246	866182.460024	45.599629
3503.066570	866151.309916	45.604634
3502.581369	866122.737048	45.609639
3502.620325	866101.653744	45.614644
3502.977936	866058.372368	45.619649
3502.640476	866042.790126	45.624653
3502.726720	866003.632517	45.629658
3502.452144	865981.629143	45.634663
3502.392564	865943.563607	45.639668
3502.787239	865925.140759	45.644673
3502.809614	865900.757005	45.649677
3502.851403	865873.747377	45.654682
3502.454666	865832.337045	45.659687
3502.721613	865801.307534	45.664692
3502.832269	865780.696964	45.669697
3502.505802	865760.546877	45.674701
3502.484889	865737.723746	45.679706
3502.691938	865710.880430	45.684711
3502.358647	865688.982795	45.689716
3502.535935	865650.390705	45.694721
3502.524095	865637.667849	45.699725
3502.863396	865597.300274	45.704730
3502.522192	865575.306392	45.709735
3502.632646	865542.261448	45.714740
3502.711494	865521.169542	45.719745
3502.412157	865494.214415	45.724749
3502.959501	865457.794316	45.729754
3502.638361	865437.739410	45.734759
3502.652988	865411.703583	45.739764
3502.750679	865375.454208	45.744769
3502.694375	865354.966832	45.749773
3502.518171	865314.585157	45.754778
3502.486972	865298.853387	45.759783
3502.636769	865275.126104	45.764788
3502.848943	865235.942765	45.769793
3502.423650	865214.932848	45.774797
3502.491113	865186.264478	45.779802
3502.368896	865166.661614	45.784807
3502.501558	865114.667576	45.789812
3502.616708	865025.177661	45.794817
3502.513947	864902.594887	45.799821
3502.797147	864691.441611	45.804826
3502.595483	864434.503528	45.809831
3502.549433	864122.439016	45.814836
3502.696898	863741.921473	45.819841
3501.849296	863303.337099	45.824845
3502.207743	862798.827629	45.829850
3502.343773	862246.495176	45.834855
3502.179535	861635.258708	45.839860
3501.821508	860934.461349	45.844865
3501.728887	860197.080882	45.849869
3501.217684	859379.168879	45.854874
3501.279269	858517.582255	45.859879
3500.866157	857582.420549	45.864884
3500.708855	856577.518487	45.869889
3500.373032	855510.892181	45.874893
3500.232731	854364.931458	45.879898
3499.845385	853150.664416	45.884903
3499.500753	851873.650260	45.889908
3499.131596	850515.555260	45.894913
3498.829882	849095.791729	45.899917
3498.612720	847582.556132	45.904922
3498.231697	846014.801483	45.909927
3497.392026	844375.674150	45.914932
3497.078915	842654.427658	45.919937
3496.493877	840853.615156	45.924941
3496.108673	838991.433408	45.929946
3495.754506	837048.927218	45.934951
3495.002629	835027.023809	45.939956
3494.632237	832945.833077	45.944961
3493.865509	830791.997965	45.949965
3493.167351	828549.982885	45.954970
3492.764071	826245.321968	45.959975
3492.052380	823866.123010	45.964980
3491.937736	821407.367151	45.969985
3490.929665	818892.995390	45.974989
3490.456418	816289.479164	45.979994
3489.779763	813612.070515	45.984999
3488.886289	810854.321286	45.990004
3488.468000	808040.284627	45.995009
3487.506586	805144.228107	46.000013
3486.627133	802176.301808	46.005018
3485.659638	799146.214476	46.010023
3484.845160	796031.958596	46.015028
3484.083018	792848.919152	46.020033
3482.658904	789612.166981	46.025037
3481.904340	786288.138228	46.030042
3481.059406	782906.800961	46.035047
3479.864414	779437.768553	46.040052
3479.368628	775913.543382	46.045057
3478.065649	772334.652683	46.050061
3477.400984	768660.235761	46.055066
3476.261159	764924.123537	46.060071
3475.106645	761127.101358	46.065076
3473.923314	757238.990551	46.070081
3472.865244	753302.901564	46.075085
3472.096634	749286.836748	46.080090
3470.758115	745206.454029	46.085095
3469.567574	741046.619279	46.090100
3468.215197	736819.008064	46.095105
3467.150536	732534.304673	46.100109
3466.119799	728175.790267	46.105114
3464.744503	723747.894809	46.110119
3463.153762	719261.024677	46.115124
3462.116208	714690.573465	46.120129
3460.599144	710065.596645	46.125133
3459.257478	705358.806397	46.130138
3458.009956	700606.145137	46.135143
3456.617203	695776.630036	46.140148
3455.019390	690874.108712	46.145153
3453.413737	685911.505976	46.150157
3452.202122	680872.006963	46.155162
3450.352230	675784.348381	46.160167
3448.774072	670619.718022	46.165172
3447.310031	665402.801248	46.170177
3445.626665	660106.503039	46.175181
3444.017778	654728.889463	46.180186
3442.256833	649313.935256	46.185191
3440.405817	643828.115017	46.190196
3439.021607	638274.520616	46.195201
3437.270064	632679.206622	46.200205
3435.697355	626995.239999	46.205210
3433.504809	621270.414379	46.210215
3431.850121	615474.546442	46.215220
3429.962092	609609.912406	46.220225
3428.236111	603702.943761	46.225229
3426.180384	597716.706205	46.230234
3424.101185	591679.520537	46.235239
3422.195417	585597.117123	46.240244
3420.303064	579427.775533	46.245249
3417.951422	573227.758070	46.250253
3416.006274	566962.157166	46.255258
3413.729549	560640.432389	46.260263
3411.294200	554257.956636	46.265268
3409.569584	547829.692793	46.270273
3406.866442	541331.717328	46.275277
3404.812781	534795.273862	46.280282
3402.620661	528204.410758	46.285287
3400.030743	521570.182867	46.290292
3397.761486	514865.309199	46.295297
3395.187509	508129.053493	46.300301
3392.699852	501329.888092	46.305306
3390.239184	494485.633186	46.310311
3387.717198	487591.827579	46.315316
3385.233794	480652.986438	46.320321
3382.493183	473674.155775	46.325325
3379.941716	466646.843020	46.330330
3377.301967	459580.556594	46.335335
3374.350154	452464.227564	46.340340
3371.870494	445310.090926	46.345345
3368.875245	438119.277752	46.350349
3366.076301	430883.152258	46.355354
3363.092674	423608.480735	46.360359
3359.871543	416290.255868	46.365364
3356.917747	408945.572901	46.370369
3353.766738	401569.987555	46.375373
3351.073611	394155.259879	46.380378
3347.923314	386717.625357	46.385383
3344.277583	379234.321169	46.390388
3341.407557	371711.160766	46.395393
3338.247055	364188.330183	46.400397
3334.916299	356612.444210	46.405402
3331.768591	349029.216955	46.410407
3328.644799	341407.326240	46.415412
3325.195612	333761.732190	46.420417
3321.479579	326093.873646	46.425421
3317.972686	318407.007015	46.430426
3313.912524	310706.276388	46.435431
3310.592786	302979.532515	46.440436
3307.387716	295254.842130	46.445441
3303.439984	287498.437835	46.450445
3299.456883	279727.526830	46.455450
3296.040754	271941.282062	46.460455
3292.403991	264160.296327	46.465460
3288.628098	256356.707464	46.470465
3284.013472	248550.076899	46.475469
3280.239920	240737.544546	46.480474
3276.314320	232911.292865	46.485479
3271.901525	225054.103525	46.490484
3268.391244	217188.075052	46.495489
3264.283483	209374.388894	46.500493
3259.764195	201551.661505	46.505498
3256.156863	193734.749766	46.510503
3251.775043	185928.755455	46.515508
3247.347554	178115.182836	46.520513
3242.746216	170318.180247	46.525517
3238.293248	162530.807400	46.530522
3233.741771	154763.860889	46.535527
3229.186226	147010.474247	46.540532
3224.312182	139258.895144	46.545537
3219.397529	131544.396286	46.550541
3214.765344	123849.795985	46.555546
3209.643972	116185.977662	46.560551
3204.265531	108556.826532	46.565556
3199.209684	100954.121979	46.570561
3193.272907	93396.819348	46.575565
3187.967468	85870.723449	46.580570
3181.962096	78401.905053	46.585575
3175.748881	70992.602342	46.590580
3169.640966	63641.824621	46.595585
3162.362015	56369.468086	46.600589
3154.631670	49179.209341	46.605594
3142.312530	42203.605014	46.610599
3121.336358	35604.062167	46.615604
3100.734853	29225.190417	46.620609
3080.297260	23161.720609	46.625613
3060.049860	17454.071961	46.630618
3039.041954	12149.553673	46.635623
3011.905678	7450.196166	46.640628
2978.877430	3384.925221	46.645633
2922.093650	539.244549	46.650637
2801.736967	303.840640	46.655642
2728.127308	307.859242	46.660647
2713.306423	307.696288	46.665652
2739.048057	283.758057	46.670657
2780.431499	282.979777	46.675661
2818.751752	280.271208	46.680666
2843.961641	286.616655	46.685671
2855.135281	286.518992	46.690676
2856.180104	287.719774	46.695681
2850.839195	276.100453	46.700685
2843.948859	280.362762	46.705690
2837.764704	276.918770	46.710695
2832.769093	276.750748	46.715700
2829.720994	264.000527	46.720705
2827.280963	272.381297	46.725709
2825.645821	268.205765	46.730714
2823.479640	258.092979	46.735719
2820.593719	267.159864	46.740724
2818.444432	256.856424	46.745729
2815.371218	263.191414	46.750733
2812.390444	262.301838	46.755738
2809.591400	254.243219	46.760743
2806.157650	253.157234	46.765748
2803.296591	255.783105	46.770753
2799.942610	259.291514	46.775757
2796.996412	260.416635	46.780762
2793.359648	259.745418	46.785767
2790.262796	259.175362	46.790772
2787.475003	238.943226	46.795777
2784.374796	246.847604	46.800781
2780.705106	247.583354	46.805786
2777.433149	246.029043	46.810791
2774.160201	249.793666	46.815796
2771.003955	249.791901	46.820801
2767.618563	246.255655	46.825805
2764.451876	254.287843	46.830810
2761.050271	242.553127	46.835815
2758.045074	254.474732	46.840820
2755.035157	245.386876	46.845825
2751.264298	251.482579	46.850829
2747.404779	249.573713	46.855834
2744.174208	243.122850	46.860839
2740.578133	249.001060	46.865844
2737.307958	239.458465	46.870849
2734.025608	252.505666	46.875853
2730.776473	236.562561	46.880858
2727.740911	231.293192	46.885863
2724.187110	228.744246	46.890868
2720.906047	232.069375	46.895873
2717.084912	234.575452	46.900877
2713.755146	228.176111	46.905882
2710.803192	239.383642	46.910887
2706.703869	234.165485	46.915892
2703.634029	236.321056	46.920897
2700.505083	236.783715	46.925901
2696.874420	229.647825	46.930906
2693.334972	229.579884	46.935911
2689.514653	241.011228	46.940916
2686.357402	225.674242	46.945921
2682.986118	229.390808	46.950925
2679.919015	234.220713	46.955930
2676.641136	228.927029	46.960935
2672.973199	224.221459	46.965940
2668.945496	223.460129	46.970945
2665.665106	228.906604	46.975949
2662.337948	223.160074	46.980954
2659.280958	218.198196	46.985959
2655.038210	218.237259	46.990964
2651.717413	214.566909	46.995969
2648.123931	225.396835	47.000973
2644.738609	224.083922	47.005978
2641.555022	216.213213	47.010983
2638.065461	229.512503	47.015988
2635.160894	216.824032	47.020993
2632.028434	216.369674	47.025997
2628.059713	215.273426	47.031002
2624.328360	219.543984	47.036007
2620.638536	220.911902	47.041012
2617.676880	208.951984	47.046017
2614.194296	212.262673	47.051021
2610.467716	219.927123	47.056026
2607.375637	209.649561	47.061031
2603.292302	205.063517	47.066036
2600.145093	209.514759	47.071041
2596.673258	212.425056	47.076045
2592.824283	217.683204	47.081050
2589.685576	216.647352	47.086055
2586.114976	216.381761	47.091060
2582.805251	210.242469	47.096065
2579.518737	215.544759	47.101069
2576.035746	212.749402	47.106074
2572.491434	217.538528	47.111079
2568.569302	216.867210	47.116084
2565.350931	198.800940	47.121089
2561.642747	210.352766	47.126093
2558.594369	221.296439	47.131098
2555.160103	205.794533	47.136103
2551.388670	209.589453	47.141108
2548.279817	208.280317	47.146113
2544.674409	198.080028	47.151117
2540.872563	200.217965	47.156122
2537.431842	200.980434	47.161127
2534.087524	200.330215	47.166132
2530.678958	200.043053	47.171137
2526.835633	204.439904	47.176141
2523.581027	204.270212	47.181146
2520.292573	198.832956	47.186151
2516.425288	200.070390	47.191156
2513.186413	198.617168	47.196161
2509.571864	196.394355	47.201165
2506.495532	195.785571	47.206170
2503.140065	205.079061	47.211175
2499.386890	197.360491	47.216180
2495.789114	196.615373	47.221185
2492.069253	199.483790	47.226189
2488.765044	195.418113	47.231194
2485.638977	200.201409	47.236199
2481.390586	203.167330	47.241204
2478.560910	192.280788	47.246209
2474.667847	194.094994	47.251213
2471.504836	196.478217	47.256218
2467.921108	203.360597	47.261223
2464.510287	186.991946	47.266228
2461.116694	192.080689	47.271233
2457.399950	201.221691	47.276237
2453.942665	197.712941	47.281242
2450.383695	195.367133	47.286247
2446.487029	197.122557	47.291252
2443.561794	195.668921	47.296257
2440.104955	193.567346	47.301261
2436.014426	195.144213	47.306266
2433.289133	196.639995	47.311271
2429.534891	193.211656	47.316276
2426.130972	192.384664	47.321281
2422.596162	207.110405	47.326285
2418.869265	188.405545	47.331290
2415.529256	189.426370	47.336295
2411.693077	200.471326	47.341300
2408.424573	192.214805	47.346305
2404.896750	194.509096	47.351309
2401.576404	196.882416	47.356314
2398.387662	190.797103	47.361319
2394.473535	188.489440	47.366324
2391.272495	194.012957	47.371329
2387.691982	190.315614	47.376333
2384.109744	185.204416	47.381338
2381.007008	181.065305	47.386343
2376.993694	190.090924	47.391348
2373.793184	189.513575	47.396353
2369.884515	189.749936	47.401357
2366.358673	191.350866	47.406362
2363.293687	193.281851	47.411367
2359.300515	194.784888	47.416372
2356.215483	193.910238	47.421377
2352.837161	183.426944	47.426381
2349.135330	189.475788	47.431386
2345.790345	180.483038	47.436391
2341.856985	191.005138	47.441396
2338.541078	197.728142	47.446401
2335.171040	190.555656	47.451405
2331.894954	187.550103	47.456410
2328.624464	180.443485	47.461415
2324.541299	189.748858	47.466420
2321.308743	183.393178	47.471425
2317.771026	190.445463	47.476429
2314.161076	185.639839	47.481434
2310.910843	179.792870	47.486439
2307.241158	187.755966	47.491444
2303.435858	177.609810	47.496449
2299.799489	178.613527	47.501453
2296.659575	182.335944	47.506458
2293.276502	182.055394	47.511463
2289.472358	183.536358	47.516468
2286.503018	169.906309	47.521473
2282.709021	182.845748	47.526477
2279.329347	181.517559	47.531482
2275.808479	183.257250	47.536487
2272.101767	178.529008	47.541492
2269.142712	177.730709	47.546497
2265.578461	170.240465	47.551501
2261.544423	181.629576	47.556506
2258.313980	182.055591	47.561511
2254.493827	186.133263	47.566516
2251.137195	172.673347	47.571521
2247.979880	175.031886	47.576525
2244.132872	185.005989	47.581530
2240.833799	168.838347	47.586535
2236.948349	178.059432	47.591540
2233.855054	168.120220	47.596545
2230.380616	179.885842	47.601549
2226.871099	174.154760	47.606554
2223.513316	173.950007	47.611559
2219.490232	170.964066	47.616564
2216.276241	171.223994	47.621569
2212.510266	166.954736	47.626573
2208.756916	183.831945	47.631578
2206.061692	173.197907	47.636583
2202.358255	177.657538	47.641588
2199.067542	169.317038	47.646593
2195.525170	174.705206	47.651597
2191.940001	179.200179	47.656602
2188.606081	170.847678	47.661607
2184.477593	178.673081	47.666612
2181.144652	171.950059	47.671617
2177.601960	172.231723	47.676621
2174.023638	174.395583	47.681626
2170.662819	161.510892	47.686631
2167.388001	166.450748	47.691636
2163.809326	165.079525	47.696641
2160.337690	170.648047	47.701645
2156.517983	178.339210	47.706650
2153.521211	167.634426	47.711655
2149.726550	177.130078	47.716660
2146.319047	165.859658	47.721665
2142.640849	167.512146	47.726669
2139.399220	165.565100	47.731674
2135.910221	166.070199	47.736679
2132.387313	167.314608	47.741684
2128.484357	166.614827	47.746689
2124.978009	164.002855	47.751693
2121.742203	178.479659	47.756698
2118.407137	165.361052	47.761703
2114.669971	181.925621	47.766708
2111.627731	169.341409	47.771713
2108.118180	173.518667	47.776717
2104.299104	164.614661	47.781722
2100.689265	164.400504	47.786727
2096.719187	172.391233	47.791732
2093.848891	167.192902	47.796737
2090.466443	165.227899	47.801741
2086.676208	170.489527	47.806746
2083.791685	168.693323	47.811751
2080.063283	174.403167	47.816756
2076.098981	162.547481	47.821761
2072.753854	163.007554	47.826765
2069.135209	168.336569	47.831770
2065.889770	162.545828	47.836775
2061.977919	174.449687	47.841780
2058.635498	167.881856	47.846785
2055.794347	167.871733	47.851789
2051.502406	175.607008	47.856794
2048.393963	170.181229	47.861799
2044.690391	172.565375	47.866804
2041.328834	159.823789	47.871809
2037.860626	164.065505	47.876813
2033.926704	171.836393	47.881818
2030.794427	165.877800	47.886823
2027.235601	171.590856	47.891828
2024.045194	163.089477	47.896833
2020.234493	172.708044	47.901837
2016.821673	174.049602	47.906842
2013.151549	167.778849	47.911847
2009.718402	180.179333	47.916852
2006.444147	165.165786	47.921857
2002.619809	162.341789	47.926861
1999.248317	164.418926	47.931866
1995.773992	157.510023	47.936871
1992.232668	175.052496	47.941876
1988.560426	160.389063	47.946881
1985.034970	171.792448	47.951885
1981.690074	175.120088	47.956890
1978.320529	157.759366	47.961895
1974.798119	160.903987	47.966900
1971.441256	161.639186	47.971905
1967.815278	161.908118	47.976909
1964.003823	166.788132	47.981914
1961.065286	159.774192	47.986919
1957.422842	161.590624	47.991924
1953.946844	152.996754	47.996929
1950.271246	158.732302	48.001933
1946.483265	160.620732	48.006938
1943.554938	157.582495	48.011943
1940.011741	170.550778	48.016948
1936.068924	164.437217	48.021953
1932.338028	163.467241	48.026957
1928.742364	164.099233	48.031962
1925.930304	155.341459	48.036967
1922.519554	162.000247	48.041972
1919.036422	160.488908	48.046977
1915.352920	164.211150	48.051981
1911.773192	154.806410	48.056986
1908.436760	154.175453	48.061991
1904.663947	161.044622	48.066996
1901.003737	157.164082	48.072001
1897.887579	158.344832	48.077005
1893.808603	159.481353	48.082010
1890.725157	156.683870	48.087015
1887.366786	162.528096	48.092020
1884.044030	164.768354	48.097025
1880.417339	155.538347	48.102029
1876.437931	153.427796	48.107034
1873.377888	154.421096	48.112039
1869.720234	157.291134	48.117044
1866.202449	148.909474	48.122049
1863.111883	151.849638	48.127053
1859.246708	151.439058	48.132058
1856.028372	143.902683	48.137063
1852.170166	154.976881	48.142068
1848.789282	151.356714	48.147073
1845.103499	152.498779	48.152077
1841.393106	159.324924	48.157082
1838.147383	146.195362	48.162087
1834.682042	147.015078	48.167092
1831.125081	151.239030	48.172097
1827.552854	157.462974	48.177101
1824.106275	160.661482	48.182106
1820.867842	148.837113	48.187111
1817.504759	146.598363	48.192116
1813.722008	157.267816	48.197121
1810.337939	157.394489	48.202125
1806.237006	155.443591	48.207130
1803.394812	149.543813	48.212135
1799.698882	157.250689	48.217140
1796.275638	153.907716	48.222145
1792.364357	153.141308	48.227149
1788.876740	156.916336	48.232154
1785.716485	153.743448	48.237159
1782.109733	151.185029	48.242164
1778.814418	152.641928	48.247169
1775.344104	150.564190	48.252173
1771.284531	156.051104	48.257178
1768.415593	153.285168	48.262183
1764.789686	150.954301	48.267188
1761.328624	162.012098	48.272193
1757.770304	157.610049	48.277197
1754.004789	156.278490	48.282202
1750.829133	152.439586	48.287207
1747.021189	157.374435	48.292212
1743.649577	154.763190	48.297217
1739.983327	153.450370	48.302221
1736.112358	156.470992	48.307226
1733.252796	153.182949	48.312231
1729.663838	159.240606	48.317236
1726.028251	148.859549	48.322241
1722.484769	146.211790	48.327245
1718.928030	150.361191	48.332250
1715.719204	149.037548	48.337255
1712.034704	155.285250	48.342260
1708.594337	149.665909	48.347265
1705.516991	143.960353	48.352269
1701.353319	143.706175	48.357274
1698.429718	142.238925	48.362279
1694.300318	157.335400	48.367284
1690.764880	155.996468	48.372289
1687.684825	152.894860	48.377293
1684.182818	153.506629	48.382298
1680.579377	156.510526	48.387303
1677.119315	161.123915	48.392308
1673.890525	152.568567	48.397313
1670.343136	151.324769	48.402317
1666.525890	148.255183	48.407322
1663.160624	142.737535	48.412327
1659.297221	144.686207	48.417332
1655.848326	152.145951	48.422337
1652.630154	149.768135	48.427341
1649.360316	152.653196	48.432346
1645.836502	148.268825	48.437351
1641.930055	149.562749	48.442356
1638.704982	145.715714	48.447361
1635.389084	144.821072	48.452365
1631.237321	143.545932	48.457370
1628.477996	145.154141	48.462375
1624.293342	149.844460	48.467380
1621.011924	149.314931	48.472385
1617.678089	143.874809	48.477389
1613.995590	151.178997	48.482394
1610.258107	144.425191	48.487399
1606.899676	145.428495	48.492404
1603.581762	152.376442	48.497409
1600.233508	144.999865	48.502413
1596.256939	142.483362	48.507418
1593.467244	142.578089	48.512423
1589.655242	147.994638	48.517428
1585.847258	141.357883	48.522433
1582.652899	145.488746	48.527437
1578.930928	149.018870	48.532442
1575.327815	142.670723	48.537447
1571.936986	139.589369	48.542452
1568.606127	132.134566	48.547457
1564.975443	140.384155	48.552461
1561.110778	149.318302	48.557466
1558.113234	134.271483	48.562471
1554.604567	141.135535	48.567476
1550.775595	139.969539	48.572481
1547.459155	137.450759	48.577485
1544.084029	144.876874	48.582490
1540.623317	139.294185	48.587495
1537.496729	140.314088	48.592500
1533.539335	145.967040	48.597505
1529.564039	138.295514	48.602509
1526.274909	146.767927	48.607514
1522.868764	148.316922	48.612519
1519.353189	142.422640	48.617524
1516.133012	141.994562	48.622529
1512.581569	140.801681	48.627533
1509.047266	147.308281	48.632538
1505.846445	144.703526	48.637543
1501.883985	141.835486	48.642548
1498.256576	140.939929	48.647553
1495.037806	139.190651	48.652557
1491.316861	139.459262	48.657562
1487.862014	131.637638	48.662567
1484.631721	142.953662	48.667572
1481.412980	140.197175	48.672577
1477.537124	132.006056	48.677581
1473.589744	147.833733	48.682586
1470.550262	145.279107	48.687591
1466.471314	145.818447	48.692596
1463.320719	144.912596	48.697601
1460.017078	141.341136	48.702605
1456.156711	139.338761	48.707610
1452.977719	135.852877	48.712615
1449.292419	141.307201	48.717620
1445.836992	138.725229	48.722625
1442.540301	136.065324	48.727629
1438.893351	144.672504	48.732634
1435.746436	141.738810	48.737639
1432.396817	145.769921	48.742644
1428.467976	149.982407	48.747649
1424.602991	138.197588	48.752653
1420.980319	149.069763	48.757658
1418.181701	146.036090	48.762663
1414.682270	139.509719	48.767668
1410.903588	139.243087	48.772673
1407.602393	146.187407	48.777677
1403.695325	143.113355	48.782682
1400.046021	131.108605	48.787687
1396.711980	138.593933	48.792692
1393.615110	143.173338	48.797697
1390.053346	136.064882	48.802701
1386.092261	139.956924	48.807706
1382.872053	131.821518	48.812711
1379.330769	138.858421	48.817716
1375.525511	136.660523	48.822721
1372.177245	143.033458	48.827725
1368.765985	138.901260	48.832730
1365.403861	137.635171	48.837735
1361.650209	139.498454	48.842740
1358.389838	132.895718	48.847745
1354.997795	137.159252	48.852749
1351.427303	134.532435	48.857754
1347.696121	137.733123	48.862759
1344.083339	137.731185	48.867764
1340.960757	130.712593	48.872769
1337.532101	141.034936	48.877773
1333.882493	138.693536	48.882778
1330.669967	139.176023	48.887783
1326.433771	135.227376	48.892788
1323.166140	135.441126	48.897793
1320.200902	139.234529	48.902797
1316.282364	134.684984	48.907802
1312.855229	130.214062	48.912807
1309.184041	136.055701	48.917812
1305.776451	131.798033	48.922817
1302.669768	124.640287	48.927821
1298.732294	137.369421	48.932826
1295.041365	131.946154	48.937831
1291.634610	130.695391	48.942836
1288.124906	136.791164	48.947841
1284.967995	135.697235	48.952845
1281.072475	130.033104	48.957850
1277.837476	124.068378	48.962855
1274.186709	127.576503	48.967860
1270.787714	130.459880	48.972865
1267.482666	120.339171	48.977869
1263.545737	129.307180	48.982874
1260.272702	123.753494	48.987879
1256.816305	140.540516	48.992884
1253.196991	137.115526	48.997889
1249.538875	130.793132	49.002893
1245.809749	130.548637	49.007898
1242.830823	129.098328	49.012903
1239.375034	128.092121	49.017908
1235.782874	129.679966	49.022913
1232.449565	135.200387	49.027917
1228.534870	133.127466	49.032922
1225.247843	125.207872	49.037927
1221.710904	130.288352	49.042932
1217.968689	139.490816	49.047937
1214.888432	130.085431	49.052941
1210.863151	130.987712	49.057946
1207.715059	127.931240	49.062951
1204.448972	129.811926	49.067956
1200.922984	131.393002	49.072961
1197.478516	122.022981	49.077965
1193.363717	134.469317	49.082970
1190.025619	125.276883	49.087975
1186.396350	136.733035	49.092980
1183.160138	139.707770	49.097985
1179.988269	122.501223	49.102989
1176.016545	127.262294	49.107994
1172.598928	124.348089	49.112999
1169.277873	129.574466	49.118004
1165.678236	133.850152	49.123009
1162.417761	121.959542	49.128013
1158.556201	141.195466	49.133018
1154.867008	126.592687	49.138023
1151.590392	124.901372	49.143028
1147.991667	128.014602	49.148033
1144.696006	124.974088	49.153037
1140.894062	130.777675	49.158042
1137.481017	115.766167	49.163047
1133.878942	127.122539	49.168052
1130.878463	129.555716	49.173057
1127.506107	123.143956	49.178061
1123.757675	129.479214	49.183066
1120.343967	122.082875	49.188071
1116.871694	128.581263	49.193076
1112.989964	124.147183	49.198081
1109.562231	129.228632	49.203085
1105.865740	125.376466	49.208090
1102.661473	131.129809	49.213095
1098.753845	128.779957	49.218100
1095.162695	134.013154	49.223105
1091.818034	123.166623	49.228109
1088.502997	131.363761	49.233114
1085.428150	127.689245	49.238119
1081.858343	128.646967	49.243124
1078.327378	127.135304	49.248129
1075.152009	128.200287	49.253133
1071.144867	128.670285	49.258138
1067.605349	124.122041	49.263143
1064.081948	121.385058	49.268148
1060.031859	115.605006	49.273153
1057.100315	123.029521	49.278157
1053.610418	127.315166	49.283162
1050.077689	124.263799	49.288167
1046.590274	127.008232	49.293172
1042.788772	124.148329	49.298177
1039.197149	121.604592	49.303181
1035.952787	126.919216	49.308186
1032.574324	110.955465	49.313191
1028.996264	115.339769	49.318196
1025.527696	129.455801	49.323201
1022.454305	122.337954	49.328205
1018.672472	126.382602	49.333210
1015.766170	119.658841	49.338215
1011.546132	129.240413	49.343220
1007.564590	131.430368	49.348225
1004.479982	127.639122	49.353229
1000.596770	134.562529	49.358234
997.501636	123.439788	49.363239
994.103043	121.412568	49.368244
990.451544	129.050504	49.373249
987.077793	121.167746	49.378253
983.342380	126.165579	49.383258
979.837829	122.074973	49.388263
976.378524	130.841676	49.393268
972.730400	128.697668	49.398273
969.898134	124.222388	49.403277
966.168125	134.357206	49.408282
962.721340	131.306498	49.413287
959.002582	133.620183	49.418292
955.294923	131.608186	49.423297
951.820281	128.028692	49.428301
948.353446	132.326585	49.433306
944.999096	125.025756	49.438311
941.566542	121.925550	49.443316
937.877179	133.872520	49.448321
934.472899	120.272875	49.453325
930.663351	129.801035	49.458330
927.275418	120.078534	49.463335
923.908705	120.069587	49.468340
920.735556	126.464178	49.473345
916.901134	112.768547	49.478349
913.486284	123.027301	49.483354
909.960112	127.775095	49.488359
906.417011	115.797063	49.493364
902.868673	123.506210	49.498369
899.565408	115.604964	49.503373
895.718469	131.371030	49.508378
892.315007	121.461683	49.513383
888.668806	125.623520	49.518388
885.073482	123.477169	49.523393
882.117777	123.314437	49.528397
878.701561	123.011984	49.533402
875.012150	115.501412	49.538407
871.701387	123.288506	49.543412
867.766753	118.358614	49.548417
864.303612	116.350065	49.553421
860.817749	121.894979	49.558426
857.433673	115.431904	49.563431
853.766256	117.827167	49.568436
850.364219	112.933528	49.573441
847.312402	114.444737	49.578445
842.878042	118.627641	49.583450
839.578310	111.256895	49.588455
836.089082	106.908131	49.593460
832.566634	119.279457	49.598465
829.649645	115.898903	49.603469
826.069762	116.269246	49.608474
822.586017	115.257530	49.613479
819.066162	126.196568	49.618484
815.025478	125.443725	49.623489
812.013011	118.673538	49.628493
808.441985	124.147327	49.633498
804.994167	125.256378	49.638503
801.392861	113.256499	49.643508
797.572092	122.312609	49.648513
794.455100	118.824065	49.653517
790.726201	109.941512	49.658522
787.055775	111.943047	49.663527
783.730127	120.232710	49.668532
780.118595	119.414834	49.673537
776.885951	110.737333	49.678541
773.450131	116.433676	49.683546
769.841908	114.294095	49.688551
766.471934	111.755758	49.693556
762.762270	121.818481	49.698561
759.317272	114.559052	49.703565
755.760215	126.171481	49.708570
752.230947	123.871837	49.713575
748.655804	121.540909	49.718580
745.214616	118.076428	49.723585
741.728606	117.314190	49.728589
738.274661	113.967859	49.733594
734.850568	109.301941	49.738599
731.165290	112.955906	49.743604
727.611316	121.242331	49.748609
724.428918	109.309196	49.753613
720.598965	112.678863	49.758618
717.309776	109.673920	49.763623
713.971083	111.333909	49.768628
710.161563	108.157327	49.773633
706.887352	105.539654	49.778637
702.952474	113.326302	49.783642
699.737993	112.341576	49.788647
696.243572	110.778595	49.793652
692.656889	102.801670	49.798657
689.330516	100.465360	49.803661
685.325562	115.886312	49.808666
682.437335	113.872589	49.813671
678.711038	119.750060	49.818676
674.804488	111.563211	49.823681
671.568170	104.830366	49.828685
668.346958	110.267895	49.833690
665.075526	109.923303	49.838695
661.198475	105.782900	49.843700
657.422406	110.931175	49.848705
654.486792	108.438483	49.853709
650.653123	118.799256	49.858714
647.050842	112.622483	49.863719
643.778220	111.797393	49.868724
640.254801	107.916215	49.873729
636.764938	107.987654	49.878733
633.025941	114.538794	49.883738
629.430747	98.818886	49.888743
626.301389	111.234436	49.893748
622.607755	112.095395	49.898753
619.291726	103.649486	49.903757
615.590842	117.805779	49.908762
612.382618	113.951805	49.913767
608.472202	107.624173	49.918772
604.900389	109.040818	49.923777
601.474579	109.824726	49.928781
597.724904	114.782595	49.933786
594.558577	116.891905	49.938791
591.321229	115.104728	49.943796
587.508790	116.887001	49.948801
584.625786	110.220089	49.953805
580.500631	116.287753	49.958810
577.053766	106.414882	49.963815
573.702025	107.063616	49.968820
569.945767	110.719982	49.973825
566.573871	107.166632	49.978829
563.451797	111.859068	49.983834
559.693625	109.933326	49.988839
556.018863	101.336467	49.993844
552.503630	114.998542	49.998849
549.241087	106.087601	50.003853
545.235608	112.429128	50.008858
541.947833	112.302429	50.013863
538.683337	110.338828	50.018868
534.661545	117.883459	50.023873
531.690330	110.765468	50.028877
528.170142	105.754301	50.033882
524.762102	109.473460	50.038887
520.721329	112.127907	50.043892
517.455818	117.917814	50.048897
514.096615	111.264628	50.053901
510.897520	103.633008	50.058906
507.034570	111.067311	50.063911
503.438256	110.301612	50.068916
500.087415	113.184291	50.073921
496.809412	112.370267	50.078925
492.870152	112.832710	50.083930
489.754618	108.022795	50.088935
485.894044	110.648442	50.093940
482.114870	112.327225	50.098945
478.918696	107.737470	50.103949
475.552981	112.244924	50.108954
472.276415	112.201277	50.113959
468.332879	106.531456	50.118964
464.666280	113.982834	50.123969
461.624511	114.172071	50.128973
458.140603	112.906310	50.133978
454.460306	106.194029	50.138983
451.319582	107.438029	50.143988
447.485557	111.987481	50.148993
443.803166	110.393848	50.153997
440.189770	111.390276	50.159002
437.050020	109.308626	50.164007
433.338143	117.005508	50.169012
430.008493	116.751043	50.174017
426.493817	105.243949	50.179021
422.758635	109.191569	50.184026
419.420844	104.762052	50.189031
416.072168	108.432592	50.194036
412.287201	117.520370	50.199041
409.081819	110.901609	50.204045
405.192322	118.277046	50.209050
401.964269	109.694608	50.214055
398.859879	112.748317	50.219060
395.120039	117.612369	50.224065
391.398557	102.472252	50.229069
387.835189	117.090995	50.234074
384.308613	110.668086	50.239079
381.209172	107.184250	50.244084
377.204333	109.480242	50.249089
374.264103	105.321619	50.254093
370.271146	102.188532	50.259098
366.331597	108.745248	50.264103
363.360082	108.077149	50.269108
359.776657	113.933198	50.274113
356.686907	100.119640	50.279117
352.875763	107.611797	50.284122
349.294390	103.643568	50.289127
345.993832	98.115108	50.294132
342.304046	107.009382	50.299137
338.917742	102.882385	50.304141
335.011849	106.920294	50.309146
331.823662	100.126482	50.314151
328.385113	97.667337	50.319156
324.688182	100.028445	50.324161
321.586299	105.717795	50.329165
318.123170	106.393054	50.334170
314.580173	109.409895	50.339175
310.845990	107.036399	50.344180
307.266954	112.060980	50.349185
304.121102	108.492531	50.354189
300.530363	110.013986	50.359194
296.813689	105.583344	50.364199
293.307112	105.622305	50.369204
289.697043	110.525347	50.374209
286.403905	103.173315	50.379213
282.689692	106.681271	50.384218
279.100204	103.625544	50.389223
275.557389	104.384870	50.394228
272.343433	107.424241	50.399233
268.946923	95.086695	50.404237
265.212288	108.506043	50.409242
261.466539	108.643031	50.414247
258.071121	105.700633	50.419252
254.561584	108.065315	50.424257
251.916371	103.187009	50.429261
248.107452	104.908606	50.434266
244.104593	108.263093	50.439271
240.903070	105.838192	50.444276
236.562740	108.592803	50.449281
233.884580	98.696800	50.454285
230.210847	115.555909	50.459290
226.627201	104.835749	50.464295
223.468651	101.312092	50.469300
219.787889	112.040973	50.474305
216.299987	102.332106	50.479309
212.636013	106.895440	50.484314
209.111745	111.714090	50.489319
205.910296	107.129569	50.494324
202.227692	110.021411	50.499329
199.059010	106.216667	50.504333
195.150758	116.735771	50.509338
191.891708	103.684269	50.514343
188.455584	99.568014	50.519348
184.540422	105.887596	50.524353
181.384677	100.573679	50.529357
177.963617	109.141997	50.534362
174.184889	104.880398	50.539367
170.569973	102.697841	50.544372
166.801030	106.731182	50.549377
163.913710	99.209656	50.554381
160.206823	103.162675	50.559386
156.778355	108.723469	50.564391
153.302269	109.293458	50.569396
149.396255	109.690129	50.574401
146.166367	96.641148	50.579405
142.592701	104.180393	50.584410
138.962880	107.685154	50.589415
135.156279	103.311384	50.594420
132.286935	112.222927	50.599425
129.108196	100.680627	50.604429
125.275576	109.519585	50.609434
121.844612	103.937122	50.614439
118.313109	100.810762	50.619444
113.974489	107.933020	50.624449
111.150161	98.742506	50.629453
107.635409	98.233001	50.634458
104.382353	105.022405	50.639463
101.179496	98.038219	50.644468
96.914586	104.294025	50.649473
93.615224	103.056225	50.654477
89.964082	114.709354	50.659482
86.521810	107.516764	50.664487
83.212686	102.992794	50.669492
79.757894	102.827995	50.674497
76.254176	99.850992	50.679501
72.653489	99.720616	50.684506
68.840836	100.850590	50.689511
65.655399	101.576769	50.694516
61.572520	107.663744	50.699521
58.679831	105.231658	50.704525
54.822143	104.425750	50.709530
51.289955	105.726566	50.714535
47.862925	103.800129	50.719540
44.612954	112.441447	50.724545
41.780475	89.541332	50.729549
37.773445	101.437727	50.734554
33.759952	97.698407	50.739559
30.462303	98.442600	50.744564
26.697629	99.907831	50.749569
23.635250	99.156349	50.754573
20.144429	103.004048	50.759578
16.502911	96.870264	50.764583
13.436886	92.015231	50.769588
9.349040	101.456575	50.774593
6.207449	101.357586	50.779597
2.613250	110.266487	50.784602