Mon Mar 08 20:06:27 2021

Number of Points = 14582

Depth (nm)	Load (N)	Time (s)
-0.998072	90.733072	0.000000
-1.063964	83.404911	0.005005
-1.811399	45.405505	0.010010
-3.026820	-11.622514	0.015014
-7.770199	-17.526555	0.020019
-12.795167	-21.315289	0.025024
-18.497419	-12.695114	0.030029
-23.040958	-12.396199	0.035034
-26.747648	-32.567161	0.040038
-30.678770	-19.421702	0.045043
-34.188898	-20.378768	0.050048
-37.677377	-7.348044	0.055053
-41.262270	-13.805784	0.060058
-44.813569	-20.688311	0.065062
-48.894139	-12.263668	0.070067
-52.169889	-20.251346	0.075072
-55.999044	-10.710977	0.080077
-60.118862	-7.336955	0.085082
-63.959070	-7.695741	0.090086
-67.864805	-8.004648	0.095091
-71.598598	-21.991613	0.100096
-75.418283	-12.436958	0.105101
-79.034994	0.209036	0.110106
-82.590188	-23.754640	0.115110
-86.560387	-7.756675	0.120115
-90.362835	-8.933512	0.125120
-94.185615	-17.171306	0.130125
-97.861503	-14.684842	0.135130
-101.264134	-13.826682	0.140134
-105.480288	-2.185651	0.145139
-109.215066	-14.270742	0.150144
-112.728111	-37.048982	0.155149
-116.730654	-1.327546	0.160154
-120.361399	-22.112825	0.165158
-124.405943	-21.762454	0.170163
-127.628290	-12.105920	0.175168
-131.732662	-25.026060	0.180173
-135.569748	-15.878519	0.185178
-139.207450	-24.096881	0.190182
-143.083357	-8.536469	0.195187
-146.575180	-11.793736	0.200192
-149.948525	-19.038783	0.205197
-154.236771	-14.743670	0.210202
-157.767829	-29.229570	0.215206
-161.629197	-7.881334	0.220211
-165.584899	-22.469771	0.225216
-169.252236	-22.527992	0.230221
-173.866075	-19.339863	0.235226
-176.923862	-15.603718	0.240230
-180.963637	-13.681914	0.245235
-184.561322	-2.133136	0.250240
-188.293850	-23.986913	0.255245
-191.818225	3.077226	0.260250
-195.419604	-14.877474	0.265254
-199.504367	-13.801526	0.270259
-202.861182	-17.034524	0.275264
-206.841644	-13.040727	0.280269
-210.819851	-14.730178	0.285274
-214.502605	-21.362826	0.290278
-218.614010	-13.331930	0.295283
-222.313395	-6.688159	0.300288
-225.672166	-8.515859	0.305293
-229.422382	-9.123691	0.310298
-232.992283	-13.126825	0.315302
-237.163470	-14.129474	0.320307
-240.656295	-18.159086	0.325312
-244.453504	0.392780	0.330317
-248.298635	-13.673887	0.335322
-251.597553	-26.733388	0.340326
-255.798950	3.013834	0.345331
-259.734470	-10.833403	0.350336
-263.331853	-23.395858	0.355341
-267.593618	-19.240384	0.360346
-270.807904	-23.773262	0.365350
-274.732858	-8.826104	0.370355
-278.398444	-3.182623	0.375360
-281.843728	-15.072373	0.380365
-286.030103	-6.605233	0.385370
-289.684306	-22.624447	0.390374
-293.871828	-2.233134	0.395379
-297.559743	-9.714741	0.400384
-300.502675	-18.778546	0.405389
-304.356455	-8.633106	0.410394
-308.234527	-16.631500	0.415398
-312.728371	-11.372966	0.420403
-316.201483	-6.655793	0.425408
-320.026897	-15.509329	0.430413
-323.755008	-2.596085	0.435418
-327.334855	-25.549379	0.440422
-331.068360	8.103182	0.445427
-334.656441	-10.638672	0.450432
-338.442480	-9.739475	0.455437
-342.583541	-8.370470	0.460442
-346.405794	-9.805492	0.465446
-349.984445	0.674540	0.470451
-353.553595	-9.214832	0.475456
-357.006933	-8.304067	0.480461
-361.489902	-14.501255	0.485466
-364.686611	-23.756251	0.490470
-368.612376	-4.489895	0.495475
-372.213150	-6.083226	0.500480
-376.108830	-19.812036	0.505485
-380.135852	-16.773968	0.510490
-383.622082	-15.140459	0.515494
-387.815463	-11.872408	0.520499
-391.556864	-16.256316	0.525504
-395.105058	-20.647411	0.530509
-398.958600	-0.465363	0.535514
-402.316457	-16.299913	0.540518
-406.009541	-11.243168	0.545523
-410.307999	-20.243355	0.550528
-413.982843	-19.219879	0.555533
-417.745938	-16.504564	0.560538
-421.106787	-17.268872	0.565542
-425.202693	-11.755153	0.570547
-428.856599	-8.767117	0.575552
-432.692819	-14.528158	0.580557
-436.754556	-8.827501	0.585562
-439.976478	-25.990874	0.590566
-443.816912	-12.624331	0.595571
-447.581774	-12.027941	0.600576
-451.749095	-12.046893	0.605581
-455.347800	-13.246221	0.610586
-458.897553	-26.063520	0.615590
-462.958971	-11.028071	0.620595
-466.424250	-15.712973	0.625600
-469.808254	-23.506153	0.630605
-474.242883	-12.567599	0.635610
-477.916532	-16.700434	0.640614
-481.764767	-15.486753	0.645619
-485.353009	-21.476521	0.650624
-488.978899	-10.638707	0.655629
-493.063768	-12.450989	0.660634
-496.464282	-22.294519	0.665638
-500.484178	-7.215181	0.670643
-504.176041	-15.632454	0.675648
-507.751592	-8.099790	0.680653
-511.675729	-5.489486	0.685658
-515.558474	-18.939439	0.690662
-519.409371	-18.094249	0.695667
-522.831298	-12.774733	0.700672
-526.573258	-26.242412	0.705677
-530.528508	-14.746441	0.710682
-534.100297	-16.691055	0.715686
-537.843363	-13.307026	0.720691
-541.998154	-16.859907	0.725696
-545.262498	-15.852912	0.730701
-549.229812	-16.993223	0.735706
-552.664795	-23.694858	0.740710
-556.959981	-13.076452	0.745715
-560.515659	-18.751210	0.750720
-564.103030	-17.821894	0.755725
-568.109349	-10.321258	0.760730
-571.635458	-23.653043	0.765734
-575.583541	-20.907937	0.770739
-579.550308	-20.228631	0.775744
-583.338023	-20.517705	0.780749
-587.138390	-16.135780	0.785754
-590.570473	-17.128147	0.790758
-594.308715	-22.215493	0.795763
-598.059522	-21.540693	0.800768
-601.905232	-11.345641	0.805773
-605.910706	-10.661685	0.810778
-609.433737	-23.404168	0.815782
-613.469390	-9.630906	0.820787
-617.060623	-17.702974	0.825792
-620.737223	-17.251288	0.830797
-624.683404	-11.420563	0.835802
-628.017057	-14.610922	0.840806
-632.233170	-8.773329	0.845811
-635.950428	-4.704199	0.850816
-639.385576	-16.166108	0.855821
-643.570913	-11.183320	0.860826
-647.198700	-17.559146	0.865830
-651.313672	-12.516630	0.870835
-654.467495	-18.357935	0.875840
-658.218447	-19.668236	0.880845
-662.002316	-10.026976	0.885850
-665.618712	-20.647819	0.890854
-669.421851	-18.121243	0.895859
-673.511089	-19.222943	0.900864
-677.052349	-28.375131	0.905869
-681.080703	-11.428793	0.910874
-684.666379	-10.367114	0.915878
-688.453931	-15.938398	0.920883
-692.469744	-18.668039	0.925888
-695.624532	-27.604427	0.930893
-699.801046	-9.986314	0.935898
-703.728058	-17.274523	0.940902
-707.241813	-16.755691	0.945907
-711.330816	-12.705890	0.950912
-714.658732	-19.924240	0.955917
-718.727578	-6.979647	0.960922
-722.084260	-8.169936	0.965926
-726.236407	-34.700327	0.970931
-729.971687	-5.265028	0.975936
-733.247792	-27.979158	0.980941
-737.270429	-10.894889	0.985946
-740.941681	-18.162407	0.990950
-745.029486	-13.061002	0.995955
-748.694061	-10.572210	1.000960
-752.342077	-12.259903	1.005965
-756.226701	-9.284964	1.010970
-759.762023	-16.608864	1.015974
-763.842229	-23.322174	1.020979
-767.454016	-9.668446	1.025984
-771.367809	-11.838717	1.030989
-774.931933	-10.274187	1.035994
-778.523821	-17.749852	1.040998
-782.347253	-13.521619	1.046003
-786.161833	-12.768528	1.051008
-789.983345	-19.642975	1.056013
-794.198468	-3.503899	1.061018
-797.651928	-24.647453	1.066022
-801.363172	-21.134076	1.071027
-805.317896	-7.283570	1.076032
-808.580868	-15.202810	1.081037
-812.998990	-4.122807	1.086042
-816.256649	-25.890506	1.091046
-819.940595	-18.989728	1.096051
-824.224849	-8.836199	1.101056
-827.500906	-13.268549	1.106061
-831.472036	-12.362641	1.111066
-834.997860	-13.804829	1.116070
-838.752114	-14.217104	1.121075
-842.389281	-10.108427	1.126080
-846.157004	-23.932529	1.131085
-850.434488	-11.714409	1.136090
-854.062524	-5.073225	1.141094
-857.835416	-6.877976	1.146099
-861.806857	-21.129921	1.151104
-865.165667	-18.219937	1.156109
-869.231089	-0.706031	1.161114
-872.824930	-15.789386	1.166118
-876.604207	-13.166956	1.171123
-880.412065	-20.723040	1.176128
-884.014132	-5.785596	1.181133
-887.808249	-9.434935	1.186138
-891.339359	-22.429535	1.191142
-895.025555	-12.458220	1.196147
-899.144408	-22.268284	1.201152
-902.801235	-17.434194	1.206157
-906.802615	-8.554087	1.211162
-909.851698	-3.727262	1.216166
-913.882351	-5.016092	1.221171
-918.113957	-16.164163	1.226176
-921.848081	-22.599808	1.231181
-926.083521	-11.682849	1.236186
-928.951962	-12.889403	1.241190
-932.801259	-13.767261	1.246195
-937.030705	-7.717295	1.251200
-940.281048	-18.628003	1.256205
-944.369884	-9.508369	1.261210
-947.680813	-6.337865	1.266214
-951.556963	-16.848904	1.271219
-955.535073	-18.940775	1.276224
-959.257758	-21.521296	1.281229
-963.344353	-8.769005	1.286234
-966.645811	-16.752813	1.291238
-970.320400	-16.154261	1.296243
-974.463529	-13.465614	1.301248
-977.641656	-17.780952	1.306253
-982.169541	-11.758876	1.311258
-985.545938	-23.638020	1.316262
-989.431830	-18.830243	1.321267
-992.936826	-23.194206	1.326272
-996.886546	-26.107335	1.331277
-1001.012443	-18.959013	1.336282
-1004.049476	-22.836444	1.341286
-1008.177926	-17.553072	1.346291
-1012.286077	-12.365970	1.351296
-1015.941143	-13.739911	1.356301
-1019.680938	-14.477455	1.361306
-1023.129674	-21.188786	1.366310
-1026.983386	-13.435874	1.371315
-1030.697643	-10.954474	1.376320
-1034.509508	-19.969785	1.381325
-1038.258891	-7.774305	1.386330
-1041.725052	-15.320112	1.391334
-1045.693341	-13.342064	1.396339
-1049.647971	-19.690198	1.401344
-1053.140738	-14.454801	1.406349
-1057.066328	-1.122607	1.411354
-1061.182971	-18.387909	1.416358
-1065.014013	-12.767262	1.421363
-1068.699819	-6.630565	1.426368
-1071.705309	-21.717796	1.431373
-1075.751095	-6.806885	1.436378
-1079.528379	-11.344768	1.441382
-1083.409754	-18.704260	1.446387
-1087.208828	-11.789396	1.451392
-1091.129253	-19.273504	1.456397
-1094.939552	-16.909095	1.461402
-1098.601759	-12.322983	1.466406
-1102.045164	-7.984733	1.471411
-1105.706469	-17.840794	1.476416
-1109.749349	-26.360166	1.481421
-1113.635063	-5.027211	1.486426
-1117.267843	-11.333680	1.491430
-1120.821953	-16.181556	1.496435
-1124.889085	-20.073808	1.501440
-1128.308160	-17.421873	1.506445
-1132.431266	-4.288186	1.511450
-1136.226031	0.790659	1.516454
-1140.005195	-18.810125	1.521459
-1143.545410	-19.388602	1.526464
-1147.382144	-6.184018	1.531469
-1151.167743	-14.302971	1.536474
-1154.670533	-27.300084	1.541478
-1158.428375	1.950161	1.546483
-1162.836734	-17.209335	1.551488
-1166.293303	-19.439466	1.556493
-1169.949267	-13.838779	1.561498
-1173.416860	-0.283235	1.566502
-1177.444585	-22.348160	1.571507
-1181.214917	-18.148290	1.576512
-1184.690151	-21.736196	1.581517
-1188.984678	-6.372187	1.586522
-1192.425071	-7.680856	1.591526
-1196.026751	-22.346119	1.596531
-1200.222523	-17.354396	1.601536
-1204.083123	-6.700344	1.606541
-1207.667240	-13.408653	1.611546
-1211.351477	-11.778521	1.616550
-1214.735376	-19.908022	1.621555
-1218.502871	-12.212755	1.626560
-1222.405968	-28.736104	1.631565
-1226.863056	0.198791	1.636570
-1230.491714	-13.421409	1.641574
-1234.040458	-22.710264	1.646579
-1237.714331	-28.300388	1.651584
-1240.828472	-45.230596	1.656589
-1245.244100	-0.297696	1.661594
-1248.623813	-21.878021	1.666598
-1252.711888	-20.528526	1.671603
-1256.985628	-3.925200	1.676608
-1260.384458	-20.368345	1.681613
-1263.969863	-40.892350	1.686618
-1267.586378	2.898829	1.691622
-1271.427645	-24.727202	1.696627
-1275.239009	-5.091523	1.701632
-1278.676265	-9.961006	1.706637
-1283.048517	0.451805	1.711642
-1286.419451	-48.662511	1.716646
-1290.350847	-9.335352	1.721651
-1293.687735	-24.649892	1.726656
-1297.778741	-15.392149	1.731661
-1301.500265	-12.762518	1.736666
-1305.528612	-11.763080	1.741670
-1309.079595	-21.690063	1.746675
-1313.252694	-0.295053	1.751680
-1316.577473	-16.005708	1.756685
-1320.668907	-13.460334	1.761690
-1324.071392	-11.985495	1.766694
-1327.699952	-15.351542	1.771699
-1331.744433	1.664612	1.776704
-1335.150219	-14.484016	1.781709
-1339.007219	-10.217989	1.786714
-1343.144020	-15.565132	1.791718
-1346.513642	-24.068838	1.796723
-1350.877127	-24.524686	1.801728
-1353.985945	-9.960412	1.806733
-1357.908943	-3.205043	1.811738
-1361.876551	-13.705444	1.816742
-1365.451185	-30.282675	1.821747
-1369.405128	6.905354	1.826752
-1372.746470	-17.851874	1.831757
-1376.561088	-12.860931	1.836762
-1380.435195	-13.510166	1.841766
-1384.188787	-4.673679	1.846771
-1388.498094	-8.684375	1.851776
-1391.948076	-17.427440	1.856781
-1395.680078	-6.768448	1.861786
-1399.262059	-11.939400	1.866790
-1402.942582	-20.655001	1.871795
-1406.858096	-7.095248	1.876800
-1410.464610	-2.530188	1.881805
-1414.400712	-5.985624	1.886810
-1418.329260	-3.696369	1.891814
-1421.862328	-7.914839	1.896819
-1425.856362	-8.030759	1.901824
-1429.534813	-15.037390	1.906829
-1433.129177	-8.449620	1.911834
-1436.858560	-7.155650	1.916838
-1440.243018	-16.000583	1.921843
-1444.622441	-6.702722	1.926848
-1448.000831	-18.347449	1.931853
-1452.060600	-9.832391	1.936858
-1455.966917	-12.701218	1.941862
-1459.544982	-18.714711	1.946867
-1463.555618	-8.815180	1.951872
-1467.074089	-14.972233	1.956877
-1470.708329	-20.341260	1.961882
-1474.518649	-12.411681	1.966886
-1478.164424	-24.240603	1.971891
-1482.520433	-15.605533	1.976896
-1485.711055	-14.060312	1.981901
-1489.833624	-3.162037	1.986906
-1493.432526	-12.511822	1.991910
-1496.805481	-27.925901	1.996915
-1501.141456	-4.068610	2.006912
-1502.013941	-13.160373	2.016909
-1499.836381	-12.165544	2.026906
-1496.726091	-19.820460	2.036902
-1494.648220	-14.655774	2.046899
-1492.448385	-14.406552	2.056896
-1490.818502	-8.358611	2.066893
-1489.036582	-12.711059	2.076890
-1487.006681	-16.076974	2.086886
-1484.881457	-16.794671	2.096883
-1483.255431	-15.686254	2.106880
-1481.160663	-11.473134	2.116877
-1479.432237	-19.621978	2.126874
-1477.486608	-20.227235	2.136870
-1475.560048	-14.979886	2.146867
-1473.800706	-17.598313	2.156864
-1471.832923	-11.531835	2.166861
-1469.916772	-19.544954	2.176858
-1467.969997	-22.872281	2.186854
-1466.232728	-17.403580	2.196851
-1464.307500	-23.239366	2.206848
-1462.232982	-23.099515	2.216845
-1460.426097	-16.034711	2.226842
-1458.580964	-18.267419	2.236838
-1456.655261	-13.703548	2.246835
-1454.719948	-18.791000	2.256832
-1453.059421	-9.795531	2.266829
-1451.170212	-23.947535	2.276826
-1449.076773	-18.106404	2.286822
-1447.391547	-18.461539	2.296819
-1445.182049	-26.707902	2.306816
-1443.730858	-15.159109	2.316813
-1441.598127	-21.252293	2.326810
-1439.647478	-18.830132	2.336806
-1437.989972	-23.181568	2.346803
-1436.148301	-12.364704	2.356800
-1434.123523	-17.584875	2.366797
-1432.338999	-14.911918	2.376794
-1430.294200	-22.413537	2.386790
-1428.250026	-11.895906	2.396787
-1426.469276	-7.023033	2.406784
-1424.694707	-17.059614	2.416781
-1422.931311	-24.716687	2.426778
-1420.998165	-19.640859	2.436774
-1418.922186	-16.957713	2.446771
-1417.140141	-21.136455	2.456768
-1415.650702	-11.107855	2.466765
-1413.539699	-17.585929	2.476762
-1411.396528	-4.662203	2.486758
-1409.512379	-22.340473	2.496755
-1407.911821	-13.960586	2.506752
-1405.892406	-28.589680	2.516749
-1403.850123	-17.023385	2.526746
-1402.108515	-11.888457	2.536742
-1400.236972	-7.819510	2.546739
-1398.377644	-14.385170	2.556736
-1396.471103	-15.835089	2.566733
-1394.620443	-9.179832	2.576730
-1392.815129	-14.033286	2.586726
-1391.105871	-18.015636	2.596723
-1389.417474	-13.459504	2.606720
-1386.652091	-13.562797	2.616717
-1385.246500	-12.131677	2.626714
-1383.422529	-8.561904	2.636710
-1381.430654	-18.559036	2.646707
-1379.686841	-15.068003	2.656704
-1377.818731	-10.145920	2.666701
-1375.671540	-15.744033	2.676698
-1373.732041	-19.166429	2.686694
-1372.064003	-15.023835	2.696691
-1370.261942	-15.664437	2.706688
-1368.747142	-10.360555	2.716685
-1366.451372	-15.829297	2.726682
-1364.546802	-15.976341	2.736678
-1362.627151	-13.388110	2.746675
-1360.702678	-10.761178	2.756672
-1358.849607	-15.458053	2.766669
-1356.956577	-6.457090	2.776666
-1355.339811	-15.513176	2.786662
-1353.388840	-13.938822	2.796659
-1351.406433	-17.371225	2.806656
-1349.363286	-15.472173	2.816653
-1347.845596	-17.805532	2.826650
-1345.822141	-12.740931	2.836646
-1343.818493	-12.895923	2.846643
-1342.195524	-11.625875	2.856640
-1340.000465	-21.904949	2.866637
-1338.504612	-14.092414	2.876634
-1336.445082	-5.059664	2.886630
-1334.649466	-14.613277	2.896627
-1332.706249	-15.391697	2.906624
-1330.570328	-11.243435	2.916621
-1328.733855	-18.089573	2.926618
-1327.029117	-15.095891	2.936614
-1325.191381	-7.960119	2.946611
-1323.168861	-8.216001	2.956608
-1321.670838	-14.330650	2.966605
-1319.577272	-11.422874	2.976602
-1317.641622	-10.111279	2.986598
-1315.683448	-20.979216	2.996595
-1313.702993	-8.370374	3.006592
-1312.313905	-9.877926	3.016589
-1310.116175	-14.884116	3.026586
-1307.965312	-2.360952	3.036582
-1306.199545	-5.002390	3.046579
-1304.480588	-13.345383	3.056576
-1302.731227	-9.307321	3.066573
-1300.809006	-9.154003	3.076570
-1298.985920	-12.085639	3.086566
-1296.887183	-9.126567	3.096563
-1295.279308	-14.477260	3.106560
-1293.366394	-9.783311	3.116557
-1291.532219	-5.008868	3.126554
-1289.342980	-13.629202	3.136550
-1287.401822	-7.774591	3.146547
-1285.655701	-8.197770	3.156544
-1283.906531	-4.683833	3.166541
-1282.200030	-5.856929	3.176538
-1280.027890	-5.358353	3.186534
-1278.014548	-6.413194	3.196531
-1276.307587	-5.724918	3.206528
-1274.558214	-9.622037	3.216525
-1272.775495	-9.230071	3.226522
-1270.990187	-4.203072	3.236518
-1268.802647	-7.264056	3.246515
-1266.696723	-16.853069	3.256512
-1265.033932	-14.738349	3.266509
-1263.058064	-10.985957	3.276506
-1261.112771	-9.554288	3.286502
-1259.638960	-10.716973	3.296499
-1257.725332	-14.788772	3.306496
-1255.749157	-12.544206	3.316493
-1253.992786	-15.646698	3.326490
-1251.727485	-8.246147	3.336486
-1250.029388	-9.405244	3.346483
-1248.158685	-10.304612	3.356480
-1246.389758	-9.138372	3.366477
-1244.522601	-9.451424	3.376474
-1242.493431	-15.349460	3.386470
-1240.729285	-10.467462	3.396467
-1238.744700	-10.813509	3.406464
-1236.908161	-7.176157	3.416461
-1235.105965	-9.905470	3.426458
-1233.230864	-0.080528	3.436454
-1231.307481	-2.486624	3.446451
-1229.250280	-7.912331	3.456448
-1227.456641	-12.119634	3.466445
-1225.770661	-7.810862	3.476442
-1223.867896	-6.809692	3.486438
-1222.118643	-6.968081	3.496435
-1220.115065	-8.850196	3.506432
-1218.171786	-13.086171	3.516429
-1216.393948	-12.595494	3.526426
-1214.360736	-12.961931	3.536422
-1212.757389	-13.483782	3.546419
-1210.778256	-13.415278	3.556416
-1208.704443	-9.397477	3.566413
-1206.585685	-14.967212	3.576410
-1204.901940	-11.712726	3.586406
-1203.131345	-14.574317	3.596403
-1201.265671	-17.743202	3.606400
-1199.338616	-10.348475	3.616397
-1197.507703	-15.570592	3.626394
-1195.798857	-16.058788	3.636390
-1193.783557	-14.352494	3.646387
-1192.123164	-8.337621	3.656384
-1189.890380	-10.853180	3.666381
-1188.218579	-9.865551	3.676378
-1186.308665	-6.642498	3.686374
-1184.245653	-1.473553	3.696371
-1182.536036	-10.162318	3.706368
-1180.492737	-12.791226	3.716365
-1178.649057	-6.483585	3.726362
-1176.990180	-14.919506	3.736358
-1174.853337	-10.528101	3.746355
-1173.275887	-6.367702	3.756352
-1171.508300	-10.079780	3.766349
-1169.386538	-11.931816	3.776346
-1167.548184	-8.269435	3.786342
-1165.553675	-2.385355	3.796339
-1163.810436	-3.152168	3.806336
-1161.809397	-9.508239	3.816333
-1159.886428	-7.176135	3.826330
-1158.280210	-2.455104	3.836326
-1155.753566	-13.124947	3.846323
-1154.544762	-11.704831	3.856320
-1152.592030	-14.091875	3.866317
-1150.547746	-8.938851	3.876314
-1148.486719	-18.138509	3.886310
-1146.991624	-10.532537	3.896307
-1144.845402	-17.132854	3.906304
-1143.209735	-6.780094	3.916301
-1141.383960	-15.151120	3.926298
-1139.247110	-7.406240	3.936294
-1137.395765	-6.909894	3.946291
-1135.460842	-8.713065	3.956288
-1133.953993	-8.930499	3.966285
-1131.762177	-1.409123	3.976282
-1130.053576	-17.216647	3.986278
-1127.939949	-6.892966	3.996275
-1126.054108	-9.662418	4.006272
-1124.208226	-7.903700	4.016269
-1122.834155	-15.127272	4.026266
-1120.790989	-5.101762	4.036262
-1118.668486	-10.424147	4.046259
-1116.762707	-4.191116	4.056256
-1114.797905	-10.561879	4.066253
-1113.104138	-7.199986	4.076250
-1111.318074	-8.363582	4.086246
-1109.317222	-4.629257	4.096243
-1107.306038	-6.749319	4.106240
-1105.569444	-3.525313	4.116237
-1103.620581	-11.074485	4.126234
-1101.585488	-12.715243	4.136230
-1099.932577	-9.342069	4.146227
-1098.243888	-21.139306	4.156224
-1096.339125	-14.111947	4.166221
-1094.429185	-11.228269	4.176218
-1092.377397	-13.558482	4.186214
-1090.498324	-10.134639	4.196211
-1088.764416	-18.333050	4.206208
-1086.812717	-15.154489	4.216205
-1084.834426	-7.115793	4.226202
-1082.756437	-14.772436	4.236198
-1081.163670	-13.762615	4.246195
-1079.412317	-12.841312	4.256192
-1077.340550	-13.371679	4.266189
-1075.516013	-14.752965	4.276186
-1073.490283	-14.923886	4.286182
-1071.964470	-14.699082	4.296179
-1070.149980	-19.024859	4.306176
-1068.244517	-19.722817	4.316173
-1066.228364	-11.300189	4.326170
-1064.263102	-15.945319	4.336166
-1062.265190	-15.147114	4.346163
-1060.467689	-16.685105	4.356160
-1058.789950	-12.305418	4.366157
-1056.748093	-16.991211	4.376154
-1054.812406	-4.644928	4.386150
-1052.958029	-12.938369	4.396147
-1051.334970	-12.132305	4.406144
-1049.119449	-12.715636	4.416141
-1047.233536	-11.351651	4.426138
-1045.741300	-18.298839	4.436134
-1044.011076	-13.878591	4.446131
-1041.607072	-3.516001	4.456128
-1039.790413	-16.558850	4.466125
-1038.121946	-7.464844	4.476122
-1035.818819	-13.600724	4.486118
-1034.377312	-8.114368	4.496115
-1032.647220	-10.571491	4.506112
-1030.363502	-10.319456	4.516109
-1028.684653	-19.203709	4.526106
-1026.795009	-14.488440	4.536102
-1024.709946	-24.084971	4.546099
-1022.994678	-13.637487	4.556096
-1021.042281	-8.738049	4.566093
-1019.357068	-17.318600	4.576090
-1017.735045	-17.941192	4.586086
-1015.758414	-10.604748	4.596083
-1013.344797	-15.203124	4.606080
-1011.846092	-16.702770	4.616077
-1009.645268	-18.354163	4.626074
-1007.967754	-18.696696	4.636070
-1006.207426	-16.401607	4.646067
-1004.300103	-17.221381	4.656064
-1002.117135	-14.793361	4.666061
-1000.262110	-16.790474	4.676058
-998.751604	-17.635203	4.686054
-996.676310	-15.385736	4.696051
-994.957091	-24.979002	4.706048
-993.145428	-11.131887	4.716045
-991.348560	-12.646042	4.726042
-988.938495	-19.689440	4.736038
-986.993385	-26.123260	4.746035
-985.630254	-13.273289	4.756032
-983.496270	-11.775246	4.766029
-981.924150	-19.046202	4.776026
-979.993074	-10.152025	4.786022
-977.806225	-20.282656	4.796019
-976.057988	-7.566877	4.806016
-974.334237	-11.398111	4.816013
-972.360831	-18.876900	4.826010
-970.661032	-14.404365	4.836006
-968.586594	-15.032952	4.846003
-966.767686	-7.922277	4.856000
-964.719918	-5.870469	4.865997
-963.237427	-22.189598	4.875994
-960.827473	-17.265382	4.885990
-959.235995	-18.050407	4.895987
-957.208432	-25.466793	4.905984
-955.515747	-19.666889	4.915981
-953.634431	-12.861426	4.925978
-951.603294	-17.014929	4.935974
-949.898935	-12.922027	4.945971
-947.909575	-17.144632	4.955968
-945.891972	-16.516832	4.965965
-943.988765	-15.812323	4.975962
-942.660101	-19.589838	4.985958
-940.534600	-17.555174	4.995955
-938.467182	-5.572449	5.005952
-936.643423	-18.573737	5.015949
-934.582720	-29.273064	5.025946
-932.972003	-23.306892	5.035942
-931.365765	-17.848386	5.045939
-929.043834	-28.755251	5.055936
-927.351012	-15.263263	5.065933
-925.572994	-19.745724	5.075930
-923.287284	-18.333458	5.085926
-921.925367	-23.338296	5.095923
-919.914175	-16.026238	5.105920
-917.663848	-25.541746	5.115917
-916.044751	-13.634161	5.125914
-914.312821	-11.520763	5.135910
-912.187787	-12.935755	5.145907
-910.494743	-15.301612	5.155904
-908.798117	-19.398443	5.165901
-906.880590	-17.564168	5.175898
-904.683498	-14.434152	5.185894
-902.512601	-8.180164	5.195891
-900.846762	-13.078856	5.205888
-899.183105	-9.756194	5.215885
-897.324428	-18.643854	5.225882
-895.361414	-13.431815	5.235878
-893.603371	-23.591712	5.245875
-891.766591	-22.376050	5.255872
-890.010791	-20.515907	5.265869
-887.838244	-17.598252	5.275866
-886.160994	-21.178849	5.285862
-883.978531	-16.090297	5.295859
-882.135783	-18.819515	5.305856
-880.722574	-14.173210	5.315853
-878.394102	-17.704758	5.325850
-876.611585	-20.631170	5.335846
-874.564201	-15.768893	5.345843
-872.966899	-16.395328	5.355840
-871.202007	-14.481364	5.365837
-869.316716	-17.886799	5.375834
-867.197665	-10.306161	5.385830
-865.185702	-13.823415	5.395827
-863.679939	-20.895812	5.405824
-861.983651	-24.747837	5.415821
-859.789497	-15.976126	5.425818
-857.676575	-14.743003	5.435814
-856.019758	-6.295887	5.445811
-854.119059	-11.940989	5.455808
-852.208142	-13.484323	5.465805
-850.551399	-18.252061	5.475802
-848.322791	-5.199296	5.485798
-846.598483	-21.880689	5.495795
-844.672888	-8.848957	5.505792
-842.744977	-9.052988	5.515789
-841.014993	-14.675528	5.525786
-839.110134	-17.731987	5.535782
-837.123416	-17.743322	5.545779
-835.520504	-9.050750	5.555776
-833.567422	-4.429129	5.565773
-831.629075	-1.865535	5.575770
-829.755323	-12.542807	5.585766
-827.929437	-9.290230	5.595763
-825.892084	-3.908441	5.605760
-824.337496	-9.733448	5.615757
-822.003924	-23.081391	5.625754
-820.306558	-6.950211	5.635750
-818.214484	-17.103458	5.645747
-816.686984	-17.170842	5.655744
-814.784647	-6.077332	5.665741
-812.864977	-11.428614	5.675738
-811.200887	-19.214661	5.685734
-809.000661	-14.637259	5.695731
-807.238560	-16.909878	5.705728
-805.458597	-10.778036	5.715725
-803.390739	-14.413114	5.725722
-801.404923	-18.314531	5.735718
-799.861880	-15.965609	5.745715
-798.005965	-2.572188	5.755712
-795.960983	-11.683755	5.765709
-794.095821	-14.656473	5.775706
-792.118061	-14.685284	5.785702
-790.343607	-12.101778	5.795699
-788.433774	-8.095270	5.805696
-786.590512	-14.376886	5.815693
-784.889407	-12.961046	5.825690
-782.876893	-17.771390	5.835686
-780.836816	-12.971011	5.845683
-779.150868	-8.024039	5.855680
-777.223023	-10.278918	5.865677
-775.251376	-7.976371	5.875674
-773.326121	-17.214036	5.885670
-771.568837	-10.213339	5.895667
-769.663989	0.554576	5.905664
-767.933641	-2.884441	5.915661
-766.106885	-5.704169	5.925658
-763.872133	-8.248068	5.935654
-762.267378	-5.822144	5.945651
-760.528850	-0.724095	5.955648
-758.699508	-9.744336	5.965645
-756.448455	-3.788780	5.975642
-754.476656	-7.337420	5.985638
-752.939314	-4.037091	5.995635
-750.774451	-7.897614	6.005632
-749.163577	-10.824926	6.015629
-747.320039	-0.770302	6.025626
-745.022988	1.805514	6.035622
-743.403400	-8.101663	6.045619
-741.721224	-4.017683	6.055616
-739.461867	-5.296104	6.065613
-737.911249	8.725604	6.075610
-735.804020	-5.216071	6.085606
-734.049485	-4.260279	6.095603
-732.283831	-0.555922	6.105600
-730.384878	-5.629115	6.115597
-728.241607	-4.309150	6.125594
-726.349385	-7.650854	6.135590
-724.818102	-5.655239	6.145587
-722.652671	-3.536758	6.155584
-720.904504	-3.659866	6.165581
-719.082851	-5.056209	6.175578
-717.093318	-10.140706	6.185574
-715.285203	-9.281878	6.195571
-713.302999	1.718451	6.205568
-711.666832	-4.574233	6.215565
-709.558420	-8.646737	6.225562
-707.985270	-4.976335	6.235558
-705.858550	-9.795395	6.245555
-704.214632	-8.124059	6.255552
-701.940872	-8.203248	6.265549
-700.243882	-4.942602	6.275546
-698.305066	-12.218305	6.285542
-696.499654	-6.856177	6.295539
-694.787352	-5.896765	6.305536
-692.671807	-4.453924	6.315533
-690.663635	-5.359029	6.325530
-688.970920	-5.174853	6.335526
-687.310520	-9.800977	6.345523
-685.133639	-8.162680	6.355520
-683.414672	-2.393596	6.365517
-681.404007	-4.407438	6.375514
-679.969884	-9.693673	6.385510
-677.816789	-13.406998	6.395507
-675.761412	-5.983352	6.405504
-674.046839	-5.594250	6.415501
-672.098238	-11.191611	6.425498
-670.358523	-9.682388	6.435494
-668.302617	-7.770555	6.445491
-666.617060	-13.411142	6.455488
-664.837847	-10.479375	6.465485
-662.679222	-7.505598	6.475482
-660.710900	-7.247021	6.485478
-658.831808	-9.964512	6.495475
-656.815462	-13.881744	6.505472
-655.184041	-13.108317	6.515469
-653.709058	-1.570614	6.525466
-651.565848	-6.756976	6.535462
-649.599592	-8.001117	6.545459
-647.840522	-13.332931	6.555456
-645.799092	-9.730984	6.565453
-644.119308	-9.843110	6.575450
-642.030781	-11.449387	6.585446
-640.024683	-17.786910	6.595443
-638.434520	-6.779145	6.605440
-636.546044	-6.087820	6.615437
-634.381649	-20.914796	6.625434
-632.873278	-9.437677	6.635430
-630.737261	-15.429658	6.645427
-628.957010	-7.191542	6.655424
-627.205410	-13.008433	6.665421
-625.292997	-11.629390	6.675418
-623.303350	-6.099277	6.685414
-621.422028	-16.253440	6.695411
-619.939463	-3.371752	6.705408
-617.651914	-4.927701	6.715405
-615.615377	-17.648591	6.725402
-614.024808	-11.685272	6.735398
-612.160016	-7.598791	6.745395
-610.272194	-11.444932	6.755392
-608.276979	-6.654594	6.765389
-606.422096	-9.453435	6.775386
-604.485904	-8.142906	6.785382
-602.709333	-6.007983	6.795379
-601.227035	-7.073730	6.805376
-598.952706	-11.343159	6.815373
-597.012958	-10.352118	6.825370
-595.308309	-12.898020	6.835366
-593.309075	-11.393882	6.845363
-591.433443	-11.033605	6.855360
-589.356964	-5.313660	6.865357
-587.837044	-9.299953	6.875354
-585.802027	-11.653899	6.885350
-583.700923	-5.165829	6.895347
-582.102318	-10.773528	6.905344
-580.112682	-5.428099	6.915341
-578.125396	-6.265041	6.925338
-576.485470	-7.057550	6.935334
-574.760994	-7.405699	6.945331
-572.789697	-9.594730	6.955328
-570.893443	-16.767230	6.965325
-568.951628	-12.142001	6.975322
-566.993025	-10.874492	6.985318
-564.876077	-14.457216	6.995315
-563.660661	-11.991070	7.005312
-561.403119	-9.396132	7.015309
-559.534938	-4.380209	7.025306
-557.646166	0.082991	7.035302
-555.449160	-16.839530	7.045299
-554.055389	-17.600601	7.055296
-551.894753	-14.825977	7.065293
-550.299662	-21.850891	7.075290
-548.398270	-15.491936	7.085286
-546.678658	-16.464509	7.095283
-544.627456	-14.190260	7.105280
-542.780801	-17.813473	7.115277
-540.743802	-18.410446	7.125274
-538.750246	-16.801151	7.135270
-536.971496	-15.354902	7.145267
-535.346434	-18.536956	7.155264
-533.288094	-18.231075	7.165261
-531.419965	-13.736141	7.175258
-529.491813	-11.986927	7.185254
-527.407659	-21.264003	7.195251
-526.084803	-10.846577	7.205248
-523.623342	-11.321864	7.215245
-521.853239	-19.719888	7.225242
-520.288649	-19.150416	7.235238
-518.320551	-13.995693	7.245235
-516.515121	-14.582503	7.255232
-514.414817	-23.519538	7.265229
-512.561399	-12.236373	7.275226
-510.640646	-12.314262	7.285222
-508.993970	-14.674016	7.295219
-507.093544	-23.061264	7.305216
-505.007318	-16.556539	7.315213
-503.422383	-13.434157	7.325210
-501.328056	-22.787043	7.335206
-499.420274	-12.755097	7.345203
-497.576816	-16.669853	7.355200
-495.476328	-9.493226	7.365197
-493.935789	-11.185537	7.375194
-492.394209	-20.551192	7.385190
-490.091867	-3.090628	7.395187
-488.339822	-16.497001	7.405184
-486.503018	-12.536992	7.415181
-484.337834	-2.672438	7.425178
-482.550553	-13.004111	7.435174
-480.647019	-10.808849	7.445171
-479.187505	-3.381435	7.455168
-476.809379	-10.963957	7.465165
-475.320398	-1.569268	7.475162
-473.132646	-4.785879	7.485158
-471.214208	3.214008	7.495155
-469.045456	3.166019	7.505152
-467.813961	-1.423053	7.515149
-466.327185	-3.228333	7.525146
-463.634025	-8.783389	7.535142
-462.033069	3.918481	7.545139
-460.024435	-3.207159	7.555136
-458.294979	-3.819686	7.565133
-456.204972	-3.062509	7.575130
-454.315811	-9.125447	7.585126
-452.699378	-3.769255	7.595123
-450.365902	-10.342056	7.605120
-448.876928	-10.270429	7.615117
-447.092737	-4.146861	7.625114
-444.917284	-1.478703	7.635110
-443.221366	-7.327632	7.645107
-441.567606	-8.081208	7.655104
-439.803439	-0.871348	7.665101
-437.461674	-0.042254	7.675098
-435.665359	-9.598549	7.685094
-433.761875	-5.046023	7.695091
-432.137578	-7.536355	7.705088
-430.076928	-4.540401	7.715085
-428.153756	-11.311336	7.725082
-426.402456	-6.384001	7.735078
-424.572726	-7.514588	7.745075
-422.325849	-10.773749	7.755072
-420.509529	-4.977373	7.765069
-418.793556	-7.638640	7.775066
-416.953036	-13.924295	7.785062
-415.594383	-3.310412	7.795059
-413.251714	-4.409210	7.805056
-411.237967	-2.195172	7.815053
-409.130361	-3.655884	7.825050
-407.667488	-0.079761	7.835046
-405.624927	10.085495	7.845043
-403.873695	4.552998	7.855040
-401.912278	-3.193441	7.865037
-400.004430	-0.817231	7.875034
-398.264894	-5.672107	7.885030
-396.180072	-5.382966	7.895027
-394.336652	4.038877	7.905024
-392.472583	-0.625892	7.915021
-390.816546	-5.064826	7.925018
-388.781780	-7.197531	7.935014
-386.943227	2.405082	7.945011
-385.348382	-9.725694	7.955008
-383.151013	-8.030390	7.965005
-381.355731	12.094264	7.975002
-379.283316	-5.177701	7.984998
-377.373070	-5.926394	7.994995
-375.506465	-3.027298	8.004992
-373.768611	-3.607950	8.014989
-372.262179	-20.060108	8.024986
-369.789361	-2.618725	8.034982
-368.169095	-6.358820	8.044979
-366.416050	-4.058916	8.054976
-364.423174	-7.116434	8.064973
-362.598721	-16.078788	8.074970
-360.911388	-7.279333	8.084966
-358.856240	-5.248690	8.094963
-356.712713	-10.793253	8.104960
-355.036330	-7.353807	8.114957
-353.197588	-8.338945	8.124954
-351.451286	-10.228214	8.134950
-349.133817	-4.480205	8.144947
-347.376817	-18.815647	8.154944
-345.826869	1.035578	8.164941
-343.749127	-2.600699	8.174938
-341.724533	-9.040417	8.184934
-340.051608	-11.102690	8.194931
-338.152872	-5.791478	8.204928
-336.238205	-6.182447	8.214925
-334.571023	1.791357	8.224922
-332.603883	-4.444986	8.234918
-330.686724	-13.392120	8.244915
-328.804918	-11.651130	8.254912
-326.783878	-6.220494	8.264909
-325.117821	-2.487290	8.274906
-323.069532	-11.273784	8.284902
-321.261564	-9.093134	8.294899
-319.453176	-16.093546	8.304896
-317.544992	-11.146962	8.314893
-315.602348	-12.990182	8.324890
-313.829999	-13.097906	8.334886
-311.607860	-23.781489	8.344883
-309.687417	-15.154988	8.354880
-308.243022	-17.436534	8.364877
-306.392400	-15.786859	8.374874
-304.367517	-9.512134	8.384870
-302.605240	-13.751664	8.394867
-300.848519	-7.083628	8.404864
-298.564288	-13.378448	8.414861
-296.861908	-11.381439	8.424858
-294.987274	-15.199978	8.434854
-293.147398	-8.021032	8.444851
-291.240000	-4.972073	8.454848
-289.452718	-2.664945	8.464845
-287.336607	-15.219895	8.474842
-285.377299	-1.141490	8.484838
-283.640123	-12.346038	8.494835
-281.846911	-5.371198	8.504832
-280.023112	-12.805070	8.514829
-278.114025	-9.568488	8.524826
-276.363221	-6.923970	8.534822
-274.328407	-7.619837	8.544819
-272.445515	-14.867357	8.554816
-270.705489	-15.405652	8.564813
-268.663758	-9.270943	8.574810
-266.671388	-6.821279	8.584807
-264.749432	-8.059617	8.594803
-263.200419	-8.587946	8.604800
-261.548210	-9.622187	8.614797
-259.429952	-13.697463	8.624794
-257.337987	-17.144895	8.634791
-255.311674	-8.189470	8.644787
-253.645347	-13.282020	8.654784
-251.555625	-18.099530	8.664781
-249.854661	-20.380939	8.674778
-248.003726	-19.163872	8.684775
-246.191364	-19.592123	8.694771
-244.379663	-20.206570	8.704768
-242.543266	-7.889455	8.714765
-240.420215	-15.072654	8.724762
-238.881895	-12.457353	8.734759
-236.786950	-7.646287	8.744755
-234.810912	-12.841933	8.754752
-232.900700	-20.114307	8.764749
-231.187003	-6.955020	8.774746
-229.349248	-8.681966	8.784743
-227.349265	-15.619740	8.794739
-225.682521	-19.573987	8.804736
-223.851963	-9.051074	8.814733
-222.024426	-19.684247	8.824730
-219.992738	-20.486931	8.834727
-218.027689	-17.235549	8.844723
-216.447707	-13.516951	8.854720
-214.029858	-17.483691	8.864717
-212.488525	-10.365977	8.874714
-210.454612	-15.540841	8.884711
-208.623836	-8.702981	8.894707
-206.875343	-19.542991	8.904704
-205.053388	-7.855077	8.914701
-203.022771	-16.452354	8.924698
-200.807486	-17.555881	8.934695
-199.194970	-18.620060	8.944691
-197.771188	-16.033820	8.954688
-195.746120	-23.416068	8.964685
-193.502724	-16.591940	8.974682
-191.747148	-9.620495	8.984679
-189.892536	-4.123706	8.994675
-188.124034	-16.662585	9.004672
-186.257031	-11.444072	9.014669
-184.484040	-14.750552	9.024666
-182.226350	-14.555121	9.034663
-180.486040	-13.688221	9.044659
-178.734823	-13.348817	9.054656
-176.794306	-8.813037	9.064653
-174.937008	-11.970341	9.074650
-173.126250	-18.241603	9.084647
-171.459971	-10.613302	9.094643
-168.923375	-18.877629	9.104640
-167.602387	-8.609653	9.114637
-165.453271	-14.139159	9.124634
-163.694924	-19.385272	9.134631
-161.620799	-15.565493	9.144627
-160.077574	-3.001007	9.154624
-158.043366	-2.466755	9.164621
-156.203635	-1.933049	9.174618
-154.109402	-11.206718	9.184615
-152.142551	-4.259476	9.194611
-150.635562	0.751266	9.204608
-148.682517	-5.687941	9.214605
-146.758542	-1.195279	9.224602
-144.868435	-5.518253	9.234599
-143.048083	-12.182583	9.244595
-141.248037	-5.235558	9.254592
-139.414301	-2.627851	9.264589
-137.346617	-8.111187	9.274586
-135.390399	-8.003394	9.284583
-133.648425	-3.792718	9.294579
-131.801298	-7.800949	9.304576
-129.834667	-2.464079	9.314573
-128.020923	-6.166999	9.324570
-125.871552	-14.776851	9.334567
-124.447569	-13.733135	9.344563
-122.670766	-0.656443	9.354560
-120.335545	-10.671124	9.364557
-118.584947	1.661379	9.374554
-116.871236	-8.694644	9.384551
-115.040732	-11.724480	9.394547
-112.959378	-7.853706	9.404544
-111.158433	-5.321267	9.414541
-109.205383	-7.186511	9.424538
-107.296319	-7.467464	9.434535
-105.310197	-10.215822	9.444531
-103.627740	-4.895170	9.454528
-101.843065	1.601213	9.464525
-99.964697	3.766069	9.474522
-97.853283	-6.828643	9.484519
-95.778904	-3.029367	9.494515
-94.224875	-6.872399	9.504512
-92.562130	1.504909	9.514509
-90.686339	-3.278346	9.524506
-88.623928	-4.516849	9.534503
-86.682414	-1.905769	9.544499
-84.811823	-10.970035	9.554496
-82.883477	-1.836193	9.564493
-81.011299	-13.223201	9.574490
-79.361058	-5.303338	9.584487
-77.233585	-13.922289	9.594483
-75.463295	-1.056084	9.604480
-73.820187	-4.338612	9.614477
-71.947084	5.187718	9.624474
-69.739174	-10.847303	9.634471
-67.841105	-5.881524	9.644467
-65.934052	-10.799212	9.654464
-64.291621	-7.958837	9.664461
-62.359006	-12.206430	9.674458
-60.688228	-8.008025	9.684455
-58.649348	-2.366847	9.694451
-56.832463	-15.473861	9.704448
-54.694632	-3.594632	9.714445
-52.748031	-0.551729	9.724442
-51.080025	-3.026684	9.734439
-49.249915	-0.372541	9.744435
-47.201728	-3.645461	9.754432
-45.525828	1.688915	9.764429
-43.478155	-5.632099	9.774426
-41.770381	-6.731895	9.784423
-39.766065	-7.266395	9.794419
-37.892497	-9.992010	9.804416
-36.077635	-8.536933	9.814413
-34.178927	-1.337150	9.824410
-32.268868	-7.606792	9.834407
-30.619789	-5.593193	9.844403
-28.578088	-7.200952	9.854400
-26.550000	-5.342535	9.864397
-24.695346	-0.019288	9.874394
-22.986519	0.117004	9.884391
-21.177824	-4.750231	9.894387
-19.190511	3.745883	9.904384
-17.377343	3.246626	9.914381
-15.492247	0.749699	9.924378
-13.460793	-2.184230	9.934375
-11.683259	-7.580139	9.944371
-9.706794	-8.244375	9.954368
-8.117364	-17.457941	9.964365
-5.984185	-15.758366	9.974362
-4.554222	-8.264339	9.984359
-2.980880	14.368568	9.994355
-1.907169	68.689972	10.004352
-1.094600	136.344144	10.014349
0.000000	190.737809	10.019354
0.507722	248.704129	10.024359
1.271746	297.750461	10.029363
1.553436	329.834209	10.034368
1.847502	370.180456	10.039373
2.339595	402.722793	10.044378
2.472813	425.241435	10.049383
3.064867	453.679092	10.054387
2.989148	473.517315	10.059392
3.527137	484.416072	10.064397
3.467957	503.751824	10.069402
3.135547	519.587904	10.074407
3.707892	536.145417	10.079411
3.981873	551.676669	10.084416
4.098716	553.575502	10.089421
4.474708	563.121949	10.094426
4.342034	582.072150	10.099431
4.749885	587.554596	10.104435
4.516687	597.956714	10.109440
4.493607	596.976373	10.114445
4.471023	606.296268	10.119450
4.557569	601.300999	10.124455
4.951625	590.847922	10.129459
4.472045	617.233388	10.134464
4.420273	616.749615	10.139469
4.581542	613.961126	10.144474
4.510135	605.160754	10.149479
4.568404	613.538963	10.154483
4.514233	640.020620	10.159488
4.909515	654.723684	10.164493
5.072158	651.081863	10.169498
4.615954	653.100489	10.174503
5.053614	656.395769	10.179507
5.025195	667.187887	10.184512
5.399464	669.526636	10.189517
5.435840	669.326839	10.194522
5.144092	675.119588	10.199527
5.688711	664.935749	10.204531
5.444035	669.396386	10.209536
5.552025	674.888844	10.214541
5.358421	679.325569	10.219546
5.403139	670.170755	10.224551
5.791062	697.256923	10.229555
5.503450	715.199132	10.234560
5.711350	712.978761	10.239565
5.648699	717.926031	10.244570
5.571553	731.327876	10.249575
6.067854	712.086031	10.254579
6.020974	726.292000	10.259584
5.689291	720.141285	10.264589
6.043499	713.584721	10.269594
5.917847	723.121397	10.274599
5.796414	727.493011	10.279603
5.805184	729.828564	10.284608
5.950157	729.630369	10.289613
5.790277	729.630601	10.294618
5.647245	745.854606	10.299623
6.046740	751.724792	10.304627
6.212824	766.201179	10.309632
6.179777	774.182470	10.314637
6.454187	775.565781	10.319642
6.215884	776.507327	10.324647
6.495783	769.573090	10.329651
6.560656	775.313732	10.334656
6.506438	779.762949	10.339661
6.582412	784.647134	10.344666
6.359821	783.884677	10.349671
6.611717	784.998772	10.354675
6.472100	804.641062	10.359680
6.718918	802.397124	10.364685
6.796107	802.985584	10.369690
6.676540	814.352157	10.374695
6.792093	819.438194	10.379699
6.758142	818.965765	10.384704
6.881114	821.406119	10.389709
6.887374	815.264542	10.394714
6.647175	827.673788	10.399719
6.940405	825.100751	10.404723
6.780370	848.665015	10.409728
7.123133	856.997992	10.414733
7.082121	858.628734	10.419738
6.769984	869.519868	10.424743
6.922508	860.338278	10.429747
7.176280	874.573711	10.434752
7.459080	879.210479	10.439757
7.705421	894.883701	10.444762
7.556941	903.395976	10.449767
7.683151	893.562558	10.454771
7.879643	900.037608	10.459776
7.336821	895.749734	10.464781
7.486246	899.860585	10.469786
7.587783	906.536860	10.474791
7.739336	909.879407	10.479795
7.293784	917.846142	10.484800
7.565555	913.407845	10.489805
7.639048	911.000725	10.494810
7.635382	914.987764	10.499815
7.806861	934.801385	10.504819
7.936060	942.542428	10.509824
7.811818	953.624429	10.514829
8.354089	951.927853	10.519834
8.136840	962.715614	10.524839
8.319908	960.059200	10.529843
8.348065	966.174777	10.534848
8.358466	962.353733	10.539853
8.531454	963.920394	10.544858
8.293785	970.034215	10.549863
8.403435	958.279527	10.554867
8.373610	968.745667	10.559872
8.142822	976.714452	10.564877
8.605138	961.090472	10.569882
8.315243	973.887811	10.574887
8.620797	975.978952	10.579891
8.527403	994.349419	10.584896
8.522185	988.408294	10.589901
8.897106	998.369937	10.594906
8.645684	1000.762800	10.599911
8.906079	992.689861	10.604915
9.192055	997.431816	10.609920
9.201696	1003.359551	10.614925
9.152084	1005.739152	10.619930
8.839544	1017.234430	10.624935
8.613745	1010.275077	10.629939
8.981832	1004.805839	10.634944
9.094183	1004.921925	10.639949
9.204399	1008.274241	10.644954
8.751445	1021.308938	10.649959
9.203964	1034.038385	10.654963
9.193849	1039.201313	10.659968
8.908791	1053.261085	10.664973
9.082385	1036.719556	10.669978
9.139123	1048.647971	10.674983
9.597926	1054.316435	10.679987
9.491978	1054.867883	10.684992
9.536461	1063.262743	10.689997
9.846553	1079.358082	10.695002
9.570296	1088.677743	10.700007
9.936768	1088.116212	10.705011
9.962200	1087.309451	10.710016
10.095557	1088.754713	10.715021
10.224053	1088.970727	10.720026
9.875716	1087.160710	10.725031
10.026909	1075.088643	10.730035
9.895654	1095.565776	10.735040
9.812020	1093.007067	10.740045
10.332398	1090.112329	10.745050
9.630752	1098.050620	10.750055
9.847500	1100.854534	10.755059
10.063540	1102.275572	10.760064
10.118832	1111.484022	10.765069
10.165273	1096.036612	10.770074
10.343139	1107.406439	10.775079
10.283754	1109.858578	10.780083
10.397162	1126.794317	10.785088
10.178424	1142.288091	10.790093
10.675179	1146.944439	10.795098
10.424010	1145.265575	10.800103
10.659947	1141.099431	10.805107
10.418151	1148.549668	10.810112
10.447977	1148.453412	10.815117
10.403256	1139.738345	10.820122
10.501219	1148.148380	10.825127
11.049520	1148.385752	10.830131
10.510754	1155.124837	10.835136
10.589035	1174.937880	10.840141
11.024251	1170.916565	10.845146
10.779150	1173.548146	10.850151
10.956415	1171.094470	10.855155
11.118622	1161.985264	10.860160
11.244091	1166.789143	10.865165
11.131407	1167.721717	10.870170
11.114509	1178.247448	10.875175
11.366858	1175.005931	10.880179
11.251442	1172.709321	10.885184
11.111249	1173.570588	10.890189
11.282977	1195.470847	10.895194
11.425247	1217.796888	10.900199
11.321440	1210.191926	10.905203
11.321948	1213.993876	10.910208
11.632223	1222.450518	10.915213
11.505464	1215.237148	10.920218
11.498107	1212.535364	10.925223
11.611473	1208.661565	10.930227
11.485104	1206.997483	10.935232
11.692701	1217.530016	10.940237
11.815062	1217.220304	10.945242
11.851644	1231.446572	10.950247
12.251711	1241.393333	10.955251
12.402448	1234.928913	10.960256
11.986917	1232.995551	10.965261
12.140378	1219.948435	10.970266
11.818880	1230.268891	10.975271
11.997741	1230.311293	10.980275
12.106455	1250.677833	10.985280
11.846843	1250.733394	10.990285
12.231912	1247.792396	10.995290
11.876713	1249.003353	11.000295
12.255425	1247.097862	11.005299
12.444296	1251.621996	11.010304
12.496352	1249.771755	11.015309
12.609404	1245.147358	11.020314
12.175869	1255.756939	11.025319
12.889616	1271.803885	11.030323
12.839449	1288.530932	11.035328
12.701034	1279.327669	11.040333
12.982669	1284.519849	11.045338
12.689118	1289.332249	11.050343
12.660275	1290.942174	11.055347
12.985337	1286.824853	11.060352
12.792547	1287.555741	11.065357
12.949555	1281.415157	11.070362
12.905898	1290.734121	11.075367
13.249101	1283.691773	11.080371
13.408723	1282.187077	11.085376
13.468846	1287.763097	11.090381
13.607201	1284.096607	11.095386
13.607569	1284.427677	11.100391
13.272392	1279.855831	11.105395
13.411530	1282.370956	11.110400
13.669800	1279.987923	11.115405
13.857134	1272.109411	11.120410
13.178114	1271.523801	11.125415
13.354351	1262.036975	11.130419
13.627896	1272.122209	11.135424
13.736058	1287.187105	11.140429
13.796831	1275.815276	11.145434
13.642054	1285.260769	11.150439
13.536621	1288.712200	11.155443
13.719654	1293.489595	11.160448
13.631591	1291.497691	11.165453
13.771318	1295.577084	11.170458
13.525250	1304.579827	11.175463
13.768334	1293.278258	11.180467
14.063040	1293.406265	11.185472
14.156512	1297.573462	11.190477
14.098897	1294.884409	11.195482
14.074644	1293.222955	11.200487
14.063507	1291.337055	11.205491
14.072300	1298.550282	11.210496
14.220458	1292.313332	11.215501
14.377623	1285.936174	11.220506
14.144575	1294.857985	11.225511
14.085096	1304.816580	11.230515
14.325496	1314.776241	11.235520
14.290515	1314.631971	11.240525
14.693780	1316.061019	11.245530
14.578188	1322.622303	11.250535
14.771311	1312.114022	11.255539
14.783285	1321.875150	11.260544
14.751960	1311.279662	11.265549
15.114880	1311.210707	11.270554
14.741627	1321.343936	11.275559
15.073526	1325.294917	11.280563
15.109700	1318.038163	11.285568
14.892613	1326.105880	11.290573
15.161046	1316.924441	11.295578
14.625402	1328.729940	11.300583
14.861538	1316.907480	11.305587
15.070207	1328.280453	11.310592
14.701360	1325.598453	11.315597
15.102229	1324.518910	11.320602
14.900515	1335.082115	11.325607
15.170153	1325.304380	11.330611
15.002221	1317.838900	11.335616
15.223716	1351.531993	11.340621
15.541794	1344.498353	11.345626
15.655666	1349.687350	11.350631
15.524403	1350.518817	11.355635
15.475160	1354.792372	11.360640
15.684205	1359.458405	11.365645
15.895100	1357.636436	11.370650
15.596777	1351.249890	11.375655
15.584029	1341.979236	11.380659
15.800018	1358.228668	11.385664
15.862054	1364.592905	11.390669
15.806397	1345.427216	11.395674
15.937674	1358.629238	11.400679
15.795032	1357.054468	11.405683
16.033005	1370.695233	11.410688
15.994374	1357.661282	11.415693
16.175728	1345.338171	11.420698
16.256919	1349.696580	11.425703
16.542095	1351.992881	11.430707
16.860583	1345.569468	11.435712
16.142546	1332.852056	11.440717
16.240280	1334.249407	11.445722
16.371733	1343.501053	11.450727
16.626594	1341.380333	11.455731
16.476449	1340.119003	11.460736
16.196697	1338.749032	11.465741
16.641958	1345.324959	11.470746
16.315712	1357.910808	11.475751
16.438973	1363.610831	11.480755
16.053646	1351.507404	11.485760
16.246207	1361.501537	11.490765
16.281860	1355.034916	11.495770
16.214667	1368.084093	11.500775
16.726915	1370.180177	11.505779
16.736206	1385.234134	11.510784
16.834513	1389.447896	11.515789
16.954718	1382.587725	11.520794
16.903197	1395.222834	11.525799
17.205106	1393.045717	11.530803
17.125113	1394.786816	11.535808
17.186814	1397.975069	11.540813
17.207298	1383.789928	11.545818
17.290989	1385.588502	11.550823
17.580349	1393.829380	11.555827
17.266746	1384.799073	11.560832
16.937453	1401.998129	11.565837
17.176192	1403.429771	11.570842
16.857308	1397.491194	11.575847
17.005974	1390.487705	11.580851
17.457787	1399.421784	11.585856
17.236870	1423.111809	11.590861
17.999802	1410.117136	11.595866
17.695926	1421.959865	11.600871
18.013024	1415.191282	11.605875
18.024947	1416.435166	11.610880
17.497350	1411.118087	11.615885
17.870795	1408.622045	11.620890
17.829601	1421.575659	11.625895
18.064825	1408.685648	11.630899
18.021190	1416.741522	11.635904
17.982892	1433.902092	11.640909
18.070129	1416.820380	11.645914
18.090046	1417.004829	11.650919
18.291060	1410.511812	11.655923
18.435266	1404.128784	11.660928
18.380959	1414.845161	11.665933
18.249109	1387.090672	11.670938
18.326693	1398.142401	11.675943
18.209047	1409.039189	11.680947
18.512815	1400.366161	11.685952
18.557720	1406.898732	11.690957
18.506632	1404.140806	11.695962
18.577773	1416.358970	11.700967
18.763602	1414.454258	11.705971
18.481061	1413.617746	11.710976
18.464679	1422.134488	11.715981
18.612090	1412.123870	11.720986
18.602725	1418.605176	11.725991
18.632472	1418.631935	11.730995
18.666849	1409.186562	11.736000
18.911594	1419.943559	11.741005
18.733906	1402.691221	11.746010
18.704019	1418.161478	11.751015
18.807334	1409.876812	11.756019
19.020122	1410.107774	11.761024
18.569215	1427.357796	11.766029
19.046233	1434.952167	11.771034
19.315688	1441.428440	11.776039
18.827635	1438.819047	11.781043
19.581311	1437.405679	11.786048
19.447766	1447.830358	11.791053
19.656383	1432.277876	11.796058
19.439078	1441.892719	11.801063
19.393026	1438.872204	11.806067
19.513082	1435.924548	11.811072
19.386209	1444.835826	11.816077
19.473015	1428.408620	11.821082
19.563377	1442.207039	11.826087
19.622390	1444.556771	11.831091
20.247755	1442.299675	11.836096
19.927104	1441.481855	11.841101
20.053541	1435.008606	11.846106
20.145144	1440.786250	11.851111
20.008919	1436.849691	11.856115
19.993389	1437.933948	11.861120
19.713215	1445.787859	11.866125
19.998962	1447.230933	11.871130
19.885104	1430.280626	11.876135
19.629461	1443.948143	11.881139
20.107866	1442.078770	11.886144
20.020846	1434.816374	11.891149
20.122398	1441.485009	11.896154
19.927433	1450.408727	11.901159
19.863548	1440.021769	11.906163
20.322985	1448.472104	11.911168
20.263961	1466.334626	11.916173
20.593809	1452.538484	11.921178
20.773309	1463.911486	11.926183
20.778197	1467.217628	11.931187
20.736083	1465.598427	11.936192
20.549231	1458.544333	11.941197
20.544123	1452.434262	11.946202
20.535731	1470.949475	11.951207
20.463479	1472.011241	11.956211
20.944491	1473.565106	11.961216
20.704107	1478.846917	11.966221
20.867768	1474.920870	11.971226
20.933834	1473.954639	11.976231
20.879115	1470.557020	11.981235
20.976120	1473.063129	11.986240
20.888914	1475.906131	11.991245
21.452111	1472.063026	11.996250
21.091276	1471.950221	12.001255
21.081752	1470.075080	12.006259
21.493581	1467.156581	12.011264
21.106975	1480.300956	12.016269
21.286577	1468.187761	12.021274
21.296802	1475.687860	12.026279
21.011031	1467.455752	12.031283
21.182808	1478.251240	12.036288
20.928215	1486.640426	12.041293
21.154930	1489.108504	12.046298
21.364887	1507.142650	12.051303
21.371700	1500.163309	12.056307
21.714800	1496.995560	12.061312
21.255857	1493.247652	12.066317
21.330317	1479.563179	12.071322
21.144641	1491.603162	12.076327
21.687255	1485.788936	12.081331
21.523441	1481.896189	12.086336
21.221482	1488.365841	12.091341
21.625452	1470.337817	12.096346
21.198841	1476.551370	12.101351
20.868737	1485.140260	12.106355
21.438231	1482.808488	12.111360
21.349114	1489.774066	12.116365
21.338523	1480.919306	12.121370
21.579725	1484.771253	12.126375
21.582902	1480.845566	12.131379
21.587723	1478.113405	12.136384
21.566691	1487.534545	12.141389
21.935025	1474.378814	12.146394
21.713662	1483.995909	12.151399
21.321535	1479.715363	12.156403
21.636528	1476.148390	12.161408
21.553196	1484.174362	12.166413
21.530934	1470.896417	12.171418
21.365642	1455.734711	12.176423
21.329250	1447.902824	12.181427
21.469232	1444.240765	12.186432
21.045117	1442.988425	12.191437
21.436865	1436.110154	12.196442
21.037385	1447.882994	12.201447
21.116261	1468.033820	12.206451
21.359290	1480.169430	12.211456
21.285500	1482.333762	12.216461
21.156321	1492.279946	12.221466
21.520871	1484.855618	12.226471
21.458236	1483.627629	12.231475
21.674891	1470.638021	12.236480
21.118756	1472.923433	12.241485
21.449320	1459.273831	12.246490
21.282109	1458.071984	12.251495
21.208430	1457.612178	12.256499
21.383100	1471.392448	12.261504
21.650810	1463.327545	12.266509
21.345221	1445.822732	12.271514
21.171718	1450.470956	12.276519
21.300417	1435.658209	12.281523
21.385708	1438.721281	12.286528
21.096990	1438.637977	12.291533
21.470186	1452.500112	12.296538
21.605511	1468.175892	12.301543
21.607123	1470.304542	12.306547
21.513087	1455.249747	12.311552
21.645448	1428.749329	12.316557
21.636329	1440.997662	12.321562
21.199153	1454.621599	12.326567
21.165511	1429.114353	12.331571
21.272395	1433.845590	12.336576
21.096916	1451.311918	12.341581
21.357524	1447.865592	12.346586
21.408204	1448.106639	12.351591
21.540547	1441.282352	12.356595
21.443225	1442.258225	12.361600
21.351172	1449.989094	12.366605
21.425171	1445.599525	12.371610
21.348099	1445.367347	12.376615
21.311342	1440.544424	12.381619
21.631705	1437.438663	12.386624
21.475837	1453.435264	12.391629
21.512108	1442.349493	12.396634
21.433274	1437.419738	12.401639
21.189945	1450.847173	12.406643
21.310524	1452.021690	12.411648
21.140048	1447.171204	12.416653
21.770535	1446.988613	12.421658
21.424177	1439.676108	12.426663
21.418699	1445.180648	12.431667
21.522832	1440.571804	12.436672
21.161993	1455.200727	12.441677
21.558138	1457.626009	12.446682
21.503580	1451.526979	12.451687
21.281996	1444.287615	12.456691
21.344142	1433.295498	12.461696
21.004380	1439.324868	12.466701
21.452887	1448.376203	12.471706
21.609871	1443.516073	12.476711
21.379980	1450.090911	12.481715
21.635102	1443.904648	12.486720
21.201099	1431.845186	12.491725
21.335866	1439.768540	12.496730
21.371604	1420.894111	12.501735
21.062612	1426.967455	12.506739
21.274862	1440.300146	12.511744
21.355001	1429.063883	12.516749
21.387688	1420.951328	12.521754
21.423711	1434.804139	12.526759
21.343087	1446.094029	12.531763
21.369158	1436.954322	12.536768
21.240886	1433.245159	12.541773
21.561372	1437.320997	12.546778
21.004983	1442.449761	12.551783
21.396304	1438.673501	12.556787
21.533814	1438.757193	12.561792
21.367864	1434.416934	12.566797
21.753880	1438.679446	12.571802
21.418151	1432.454951	12.576807
21.665883	1427.641855	12.581811
21.882808	1428.980782	12.586816
21.495698	1442.886890	12.591821
21.689073	1440.607224	12.596826
21.477311	1438.135121	12.601831
21.551370	1431.198706	12.606835
21.365066	1436.820393	12.611840
21.442191	1433.835428	12.616845
21.333010	1411.024300	12.621850
21.194676	1412.736858	12.626855
21.193905	1419.705660	12.631859
21.695039	1425.160936	12.636864
21.551731	1420.900651	12.641869
21.294337	1405.286897	12.646874
21.258627	1407.473531	12.651879
21.532323	1408.759246	12.656883
21.202684	1399.449205	12.661888
21.262072	1411.057369	12.666893
21.298624	1409.370434	12.671898
21.207597	1406.950045	12.676903
21.187381	1408.993856	12.681907
21.361221	1408.067213	12.686912
21.446933	1417.860801	12.691917
21.299848	1415.638590	12.696922
21.121892	1427.033877	12.701927
20.990515	1430.486324	12.706931
21.462304	1438.647671	12.711936
21.203082	1444.225795	12.716941
21.484273	1445.207537	12.721946
22.017151	1451.690691	12.726951
21.309177	1433.507303	12.731955
21.099188	1416.067706	12.736960
21.158990	1415.996630	12.741965
21.696414	1418.046128	12.746970
21.093675	1423.399902	12.751975
21.381452	1425.456099	12.756979
21.545870	1410.558831	12.761984
21.321983	1417.861267	12.766989
21.310193	1398.543427	12.771994
21.347026	1430.816905	12.776999
20.940233	1418.056086	12.782003
21.105751	1422.369528	12.787008
21.512554	1449.171815	12.792013
21.267258	1450.841510	12.797018
21.201015	1450.167624	12.802023
21.485704	1445.850112	12.807027
21.601485	1444.470667	12.812032
21.483813	1444.349045	12.817037
21.453112	1418.070200	12.822042
21.307635	1419.552081	12.827047
21.340219	1420.193414	12.832051
21.425276	1427.293615	12.837056
21.549811	1415.107242	12.842061
21.600878	1409.849267	12.847066
21.521628	1430.110416	12.852071
21.495513	1418.987303	12.857075
21.521088	1405.686019	12.862080
21.211927	1407.104115	12.867085
20.991115	1428.168447	12.872090
21.505139	1421.461498	12.877095
21.097032	1416.831850	12.882099
21.249490	1428.653848	12.887104
21.285441	1425.421557	12.892109
21.409106	1419.464432	12.897114
21.043995	1406.181299	12.902119
21.030924	1434.241147	12.907123
21.526718	1412.174070	12.912128
21.374763	1427.154437	12.917133
21.355023	1422.338268	12.922138
21.677410	1403.884935	12.927143
21.451922	1424.664573	12.932147
21.467360	1431.635527	12.937152
21.355417	1433.887940	12.942157
21.169530	1421.684835	12.947162
21.387287	1431.586687	12.952167
21.258567	1446.978118	12.957171
21.539899	1429.324526	12.962176
21.328326	1436.391613	12.967181
21.203402	1426.381838	12.972186
21.460427	1429.592566	12.977191
21.310442	1435.449740	12.982195
21.536636	1421.514035	12.987200
21.566597	1421.217478	12.992205
21.310023	1432.606384	12.997210
21.332874	1432.030256	13.002215
21.725960	1426.809194	13.007219
22.027329	1410.729420	13.012224
21.375741	1422.550331	13.017229
21.383240	1413.303210	13.022234
21.560843	1399.307466	13.027239
21.170880	1395.431886	13.032243
21.308707	1397.491492	13.037248
21.136106	1402.000781	13.042253
21.410207	1400.216037	13.047258
21.546680	1409.239839	13.052263
21.269801	1404.728041	13.057267
21.321390	1392.537551	13.062272
20.981146	1404.209443	13.067277
21.418554	1421.481795	13.072282
21.537524	1423.867695	13.077287
21.122032	1420.601743	13.082291
21.312418	1406.886234	13.087296
21.261424	1429.774870	13.092301
21.312047	1431.329559	13.097306
21.403834	1434.374247	13.102311
21.527358	1431.086986	13.107315
21.629218	1413.958789	13.112320
20.984828	1405.052187	13.117325
21.347809	1409.829308	13.122330
21.330964	1422.730153	13.127335
21.336583	1405.279838	13.132339
21.120051	1407.578890	13.137344
21.302133	1435.918285	13.142349
21.352450	1437.936658	13.147354
21.368677	1422.834348	13.152359
21.431591	1445.066161	13.157363
21.430224	1432.059317	13.162368
21.477367	1411.869447	13.167373
21.289386	1427.401198	13.172378
21.234223	1408.710020	13.177383
21.083240	1416.079677	13.182387
21.031847	1417.466126	13.187392
21.400439	1449.357144	13.192397
21.658582	1433.681641	13.197402
21.645679	1429.558255	13.202407
21.147271	1454.904272	13.207411
21.343674	1408.739623	13.212416
21.283101	1425.263479	13.217421
21.151416	1452.515936	13.222426
21.464371	1425.020027	13.227431
21.231898	1453.927054	13.232435
21.708322	1421.910650	13.237440
21.275019	1417.385948	13.242445
21.256200	1419.770168	13.247450
21.415549	1415.009020	13.252455
21.109654	1406.567262	13.257459
21.218564	1422.966313	13.262464
21.491594	1439.996813	13.267469
21.052748	1438.959717	13.272474
21.667700	1434.069131	13.277479
21.483280	1425.783035	13.282483
21.139243	1432.148983	13.287488
21.161072	1422.066921	13.292493
21.140784	1421.764184	13.297498
21.684985	1443.020353	13.302503
21.438783	1437.465992	13.307507
21.345319	1435.053873	13.312512
21.283047	1416.081537	13.317517
21.337656	1405.456505	13.322522
21.372695	1422.026612	13.327527
20.992390	1436.677545	13.332531
21.679361	1420.913164	13.337536
21.197065	1424.304879	13.342541
21.483792	1435.320127	13.347546
21.513109	1407.752789	13.352551
21.040545	1423.416656	13.357555
21.065283	1431.034270	13.362560
21.544202	1423.481343	13.367565
21.664545	1438.523954	13.372570
21.290203	1439.225455	13.377575
21.067873	1412.239149	13.382579
21.592706	1423.541275	13.387584
21.316426	1425.490305	13.392589
21.133310	1421.368835	13.397594
21.566505	1406.955421	13.402599
21.272386	1417.511345	13.407603
21.581948	1403.753178	13.412608
21.483511	1417.471295	13.417613
21.078934	1409.950465	13.422618
21.036212	1408.023855	13.427623
21.273708	1437.139754	13.432627
21.438234	1423.308503	13.437632
21.124949	1428.518343	13.442637
21.149527	1430.236461	13.447642
21.581212	1442.671543	13.452647
21.419756	1464.680543	13.457651
21.433891	1446.607485	13.462656
21.477739	1421.586223	13.467661
21.512154	1425.592561	13.472666
21.738613	1408.800898	13.477671
21.529431	1418.384467	13.482675
21.669172	1408.947522	13.487680
21.774751	1415.656505	13.492685
21.576667	1425.618364	13.497690
22.051882	1415.083944	13.502695
21.515124	1401.517524	13.507699
21.198853	1386.689057	13.512704
21.347792	1382.965660	13.517709
21.138371	1384.314229	13.522714
21.334186	1389.390822	13.527719
21.137808	1411.504660	13.532723
21.714662	1410.304004	13.537728
21.399019	1400.663716	13.542733
21.313570	1388.564472	13.547738
21.348523	1384.387734	13.552743
21.187580	1381.057540	13.557747
21.420540	1382.660416	13.562752
21.503009	1377.717572	13.567757
21.524545	1382.817226	13.572762
21.700112	1392.784128	13.577767
21.498513	1381.053505	13.582771
21.524802	1380.178781	13.587776
21.290612	1384.671078	13.592781
21.320686	1396.484182	13.597786
21.382784	1380.652341	13.602791
21.115685	1390.795497	13.607795
21.224122	1390.718242	13.612800
21.159954	1388.127989	13.617805
21.252443	1383.968884	13.622810
21.167249	1386.220178	13.627815
21.107482	1381.874039	13.632819
21.426627	1390.438180	13.637824
21.289704	1383.871333	13.642829
21.181704	1389.974110	13.647834
21.410310	1380.980336	13.652839
21.198766	1383.090928	13.657843
21.233560	1375.471659	13.662848
21.053815	1405.541880	13.667853
21.498846	1410.036250	13.672858
20.967942	1407.252342	13.677863
20.862792	1448.335484	13.682867
21.295266	1420.274883	13.687872
21.624083	1432.606512	13.692877
21.489492	1411.453699	13.697882
21.346405	1432.649148	13.702887
21.263461	1432.717535	13.707891
21.330653	1416.536327	13.712896
21.386613	1421.058057	13.717901
21.503235	1431.912770	13.722906
21.716804	1426.054848	13.727911
21.184777	1422.514160	13.732915
21.608272	1415.428981	13.737920
21.498921	1413.754276	13.742925
20.955356	1396.995543	13.747930
21.327341	1396.726443	13.752935
21.397337	1426.648067	13.757939
21.376189	1415.366465	13.762944
21.152213	1400.698311	13.767949
21.300712	1427.114388	13.772954
21.558445	1430.482702	13.777959
21.357809	1423.432401	13.782963
21.445078	1402.621118	13.787968
21.550047	1405.343570	13.792973
21.477750	1402.789305	13.797978
21.383637	1390.306656	13.802983
21.151631	1391.490090	13.807987
21.603549	1400.286956	13.812992
21.408925	1385.355510	13.817997
21.477253	1400.611385	13.823002
21.637355	1402.079223	13.828007
21.030271	1389.456029	13.833011
21.287416	1388.799959	13.838016
21.015941	1393.293474	13.843021
20.921299	1392.666698	13.848026
21.175913	1388.477005	13.853031
21.294025	1413.040214	13.858035
21.261924	1436.775845	13.863040
21.035383	1424.766883	13.868045
21.118647	1441.952232	13.873050
21.581345	1403.715249	13.878055
21.019732	1447.459022	13.883059
21.505942	1419.035031	13.888064
21.420667	1450.881740	13.893069
21.235819	1416.226843	13.898074
21.591726	1444.003931	13.903079
21.348638	1423.906064	13.908083
21.473199	1419.047959	13.913088
21.364326	1437.527114	13.918093
21.877100	1431.487427	13.923098
21.646347	1408.665728	13.928103
21.139868	1421.680931	13.933107
21.446012	1409.416713	13.938112
21.379067	1397.524250	13.943117
20.899909	1403.531681	13.948122
21.003316	1407.391390	13.953127
21.159091	1410.501564	13.958131
21.348818	1422.345999	13.963136
21.392159	1442.302179	13.968141
21.443863	1459.412155	13.973146
21.543465	1427.283944	13.978151
21.342058	1420.173842	13.983155
21.559737	1419.140855	13.988160
21.448968	1411.018068	13.993165
21.582625	1412.028067	13.998170
21.478747	1410.656848	14.003175
21.285711	1411.741026	14.008179
21.344019	1407.792374	14.013184
20.989643	1415.085656	14.018189
20.869214	1421.627809	14.023207
21.382560	1415.200557	14.028224
21.191806	1408.670103	14.033242
21.224586	1429.707986	14.038259
21.697850	1437.465854	14.043277
21.487772	1435.715575	14.048295
21.416420	1407.514186	14.053312
21.228160	1416.804224	14.058330
21.596887	1422.483565	14.063347
21.720471	1438.234394	14.068365
21.237273	1426.471690	14.073383
21.811297	1432.231547	14.078400
21.433506	1429.801754	14.083418
21.311776	1431.383089	14.088435
21.513829	1422.562660	14.093453
21.537992	1445.632641	14.098471
21.627179	1452.253168	14.103488
21.511501	1450.789842	14.108506
21.327756	1433.639143	14.113523
21.515533	1458.698023	14.118541
21.565802	1447.112909	14.123559
21.744049	1452.312998	14.128576
21.673877	1445.598134	14.133594
21.377455	1442.376742	14.138611
21.581907	1451.970674	14.143629
21.427810	1463.394532	14.148647
21.586935	1441.220126	14.153664
21.515901	1452.959480	14.158682
21.453258	1467.911086	14.163699
21.699896	1479.733502	14.168717
21.405736	1485.334548	14.173735
21.454551	1475.953380	14.178752
21.456052	1492.936500	14.183770
21.504940	1489.568795	14.188787
21.874862	1481.190305	14.193805
21.978712	1529.291038	14.198823
22.112518	1490.357374	14.203840
21.763140	1508.573056	14.208858
22.103783	1526.183228	14.213875
22.086570	1504.150103	14.218893
22.162660	1531.839634	14.223911
22.126760	1514.844579	14.228928
22.153253	1497.636680	14.233946
22.110192	1502.516589	14.238963
22.250107	1500.874074	14.243981
22.330810	1477.477334	14.248999
22.017045	1489.507105	14.254016
21.509558	1503.518270	14.259034
22.187917	1488.391284	14.264051
22.437591	1521.339879	14.269069
22.136483	1525.216492	14.274087
22.567444	1519.901845	14.279104
22.311504	1519.039738	14.284122
22.275627	1519.158678	14.289139
22.515921	1533.245663	14.294157
22.309445	1511.335517	14.299175
22.424536	1504.432210	14.304192
22.398529	1520.221142	14.309210
22.332331	1509.934956	14.314227
22.647642	1513.255523	14.319245
22.391045	1512.163866	14.324263
22.316025	1489.518657	14.329280
22.380341	1520.349701	14.334298
22.535979	1510.808333	14.339315
22.687244	1509.119964	14.344333
22.469216	1509.610863	14.349351
22.381402	1501.451649	14.354368
22.605217	1514.783070	14.359386
22.801722	1514.371035	14.364403
22.546816	1494.791925	14.369421
22.069538	1502.227957	14.374439
22.689176	1508.704139	14.379456
22.740024	1519.516501	14.384474
22.736985	1531.130247	14.389491
22.953723	1514.761844	14.394509
22.531479	1529.456268	14.399527
22.729384	1519.573109	14.404544
22.779433	1519.348020	14.409562
22.736669	1520.101968	14.414579
22.901493	1526.043524	14.419597
22.628234	1533.045925	14.424615
22.799925	1513.883232	14.429632
22.692676	1527.821151	14.434650
22.258023	1523.346101	14.439667
22.595520	1522.450698	14.444685
22.557177	1516.506203	14.449703
22.734235	1511.260365	14.454720
22.668663	1536.773478	14.459738
22.814691	1524.646083	14.464755
22.791576	1515.229171	14.469773
22.534224	1544.678585	14.474791
22.972319	1538.357659	14.479808
23.336122	1539.255975	14.484826
23.212948	1556.497360	14.489843
23.458352	1545.695065	14.494861
23.095879	1531.073793	14.499879
23.108752	1539.402201	14.504896
22.918891	1526.614240	14.509914
22.800467	1544.009791	14.514931
23.145270	1550.420501	14.519949
23.121781	1553.820277	14.524967
22.999810	1558.214154	14.529984
23.423162	1550.959650	14.535002
23.084941	1541.241414	14.540019
23.075871	1543.618025	14.545037
23.125882	1554.475377	14.550055
23.257826	1544.087569	14.555072
23.132211	1552.778622	14.560090
23.043103	1557.602974	14.565107
23.323379	1553.987571	14.570125
23.027172	1549.210443	14.575143
23.156110	1549.501293	14.580160
23.323251	1555.607655	14.585178
23.163301	1579.572350	14.590195
24.127503	1562.551445	14.595213
24.173775	1532.524484	14.600231
24.670193	1528.492384	14.605248
24.841489	1523.406332	14.610266
24.782474	1510.808295	14.615283
24.648726	1488.944784	14.620301
24.281257	1469.638480	14.625319
23.897175	1457.131657	14.630336
24.312277	1455.029996	14.635354
24.230959	1452.952451	14.640371
24.340446	1434.941758	14.645389
23.980369	1422.811794	14.650407
23.956519	1416.957834	14.655424
23.792313	1415.521127	14.660442
24.074615	1419.863073	14.665459
24.132691	1411.150553	14.670477
23.812136	1410.187077	14.675495
23.458258	1418.065838	14.680512
24.018702	1426.041023	14.685530
23.668677	1413.380947	14.690547
23.807645	1411.950944	14.695565
23.615626	1409.782525	14.700583
23.774117	1402.046538	14.705600
23.998298	1397.677232	14.710618
23.663552	1418.215310	14.715635
24.016908	1409.221328	14.720653
24.007882	1415.206293	14.725671
23.958797	1416.963224	14.730688
23.822747	1399.814395	14.735706
23.679209	1413.611707	14.740723
23.708697	1405.339462	14.745741
24.099562	1421.587174	14.750759
24.169873	1433.535197	14.755776
24.368364	1428.893137	14.760794
23.928057	1419.501924	14.765811
24.302488	1417.774829	14.770829
23.821824	1419.308017	14.775847
23.728985	1432.235276	14.780864
24.168290	1442.461831	14.785882
23.863817	1444.080176	14.790899
23.987685	1444.705303	14.795917
23.976227	1439.675167	14.800935
23.797182	1442.346273	14.805952
23.966415	1452.634782	14.810970
23.918588	1469.635181	14.815987
24.303356	1464.496229	14.821005
24.573717	1472.231422	14.826023
24.162065	1475.771733	14.831040
24.346962	1494.175889	14.836058
24.294367	1476.750972	14.841075
24.355036	1493.509161	14.846093
24.295935	1485.943107	14.851111
24.188660	1492.568243	14.856128
24.634616	1485.369940	14.861146
24.279578	1485.203164	14.866163
24.427882	1489.228311	14.871181
24.562228	1493.576572	14.876199
24.406826	1492.273730	14.881216
24.634780	1480.965409	14.886234
24.428183	1493.531777	14.891251
24.519347	1478.784729	14.896269
24.277318	1498.488615	14.901287
24.407345	1505.706676	14.906304
24.778127	1515.635908	14.911322
24.469838	1527.933816	14.916339
24.775613	1527.337618	14.921357
24.817655	1528.219610	14.926375
24.602330	1529.510724	14.931392
24.930026	1521.425228	14.936410
24.703702	1522.230472	14.941427
24.614382	1528.601086	14.946445
24.572565	1523.020500	14.951463
24.674384	1516.628949	14.956480
24.986462	1513.832724	14.961498
24.796803	1524.010213	14.966515
25.028294	1515.918041	14.971533
25.434595	1508.782677	14.976551
24.992140	1513.664940	14.981568
24.979521	1507.944428	14.986586
24.959213	1507.747862	14.991603
24.803277	1524.402209	14.996621
25.040940	1538.808935	15.001639
24.984977	1547.311916	15.006656
25.756355	1551.746572	15.011674
25.219390	1539.351359	15.016691
25.334773	1527.109302	15.021709
25.405468	1521.328309	15.026727
25.198439	1518.622736	15.031744
25.419804	1503.823439	15.036762
25.176047	1506.542628	15.041779
25.191378	1508.696698	15.046797
25.411640	1510.270689	15.051815
25.356209	1522.866456	15.056832
25.428809	1506.848229	15.061850
25.343326	1518.429496	15.066867
25.529496	1522.657820	15.071885
25.574469	1509.299183	15.076903
25.137155	1522.316064	15.081920
25.333908	1538.682952	15.086938
25.524620	1545.830009	15.091955
25.751667	1548.147728	15.096973
25.687291	1543.672606	15.101991
25.609664	1543.349905	15.107008
25.903790	1528.557855	15.112026
25.562509	1519.790986	15.117043
25.579874	1509.063624	15.122061
25.744953	1499.925012	15.127079
25.566902	1512.110903	15.132096
25.539338	1514.334734	15.137114
25.956781	1522.169189	15.142131
25.709168	1522.155161	15.147149
25.323543	1520.552414	15.152167
25.768941	1541.155005	15.157184
26.127766	1538.584122	15.162202
25.845221	1542.495531	15.167219
25.980320	1546.931775	15.172237
26.047419	1535.573562	15.177255
25.664124	1524.315500	15.182272
25.959460	1534.639011	15.187290
25.869730	1542.854801	15.192307
25.942681	1541.004317	15.197325
25.917746	1551.494532	15.202343
25.659321	1543.361716	15.207360
26.192570	1530.082487	15.212378
26.378310	1544.763333	15.217395
25.970225	1539.214413	15.222413
26.116720	1544.759363	15.227431
25.940587	1555.264255	15.232448
26.043085	1545.395508	15.237466
26.307395	1547.605827	15.242483
25.953494	1549.383859	15.247501
26.281366	1538.585720	15.252519
26.158075	1543.752137	15.257536
26.354390	1542.410500	15.262554
26.080807	1546.218237	15.267571
25.545310	1548.745654	15.272589
26.169486	1541.022626	15.277607
26.118504	1541.977655	15.282624
26.118357	1552.883902	15.287642
26.845925	1555.108430	15.292659
26.293866	1547.200188	15.297677
26.614446	1559.703775	15.302695
26.340211	1553.472851	15.307712
26.351411	1543.511702	15.312730
26.501301	1543.912466	15.317747
26.264912	1558.740083	15.322765
26.702516	1559.307315	15.327783
26.747724	1568.868521	15.332800
26.964896	1561.651613	15.337818
26.598248	1548.440379	15.342835
26.573939	1561.657263	15.347853
26.309159	1549.675585	15.352871
26.267571	1560.897538	15.357888
26.834576	1566.301503	15.362906
26.771013	1581.416964	15.367923
26.923911	1577.261888	15.372941
27.069981	1572.426800	15.377959
26.978985	1569.082958	15.382976
26.712629	1568.063637	15.387994
27.079868	1571.122686	15.393011
26.923386	1564.100643	15.398029
27.208766	1555.214937	15.403047
26.960067	1543.366762	15.408064
27.222418	1530.171633	15.413082
27.329592	1523.021048	15.418099
27.074106	1534.929880	15.423117
27.438956	1528.134590	15.428135
27.117384	1529.925552	15.433152
26.857980	1537.971777	15.438170
27.418708	1529.614738	15.443187
27.135848	1533.999661	15.448205
27.494261	1534.508738	15.453223
27.342203	1531.808553	15.458240
27.278949	1524.406730	15.463258
27.421821	1531.767470	15.468275
27.216153	1535.569092	15.473293
27.495159	1524.092151	15.478311
27.156837	1536.560019	15.483328
27.066618	1529.590344	15.488346
27.152231	1530.606956	15.493363
26.844438	1538.470567	15.498381
27.373648	1520.293733	15.503399
26.932160	1522.475042	15.508416
27.209800	1528.990047	15.513434
27.588228	1526.123466	15.518451
27.079668	1530.703253	15.523469
27.445078	1514.484168	15.528487
27.224828	1531.806284	15.533504
27.107974	1528.441407	15.538522
27.676063	1549.358701	15.543539
27.580696	1553.863162	15.548557
27.859184	1559.096066	15.553575
27.653570	1546.890242	15.558592
27.789019	1545.898076	15.563610
27.912909	1529.346268	15.568627
27.409742	1531.877177	15.573645
27.317028	1534.812950	15.578663
27.376337	1551.183683	15.583680
27.554120	1559.548722	15.588698
27.622366	1556.254990	15.593715
27.450988	1568.126841	15.598733
27.778176	1554.697986	15.603751
27.603278	1554.752583	15.608768
27.539614	1562.671653	15.613786
28.084314	1545.529699	15.618803
27.858864	1551.128464	15.623821
27.966624	1544.315180	15.628839
27.896770	1553.038238	15.633856
27.984883	1571.092995	15.638874
28.234395	1572.454695	15.643891
27.954799	1580.466411	15.648909
28.159075	1570.742646	15.653927
28.181007	1580.046456	15.658944
28.069838	1579.092045	15.663962
28.383958	1585.464408	15.668979
28.210325	1584.826691	15.673997
27.939202	1570.200246	15.679015
28.406727	1560.967746	15.684032
28.221006	1561.494391	15.689050
28.289839	1564.660802	15.694067
28.227981	1566.168110	15.699085
28.439775	1579.355222	15.704103
28.592622	1571.604315	15.709120
28.103441	1566.415946	15.714138
28.592491	1562.545457	15.719155
28.356493	1564.524118	15.724173
28.272055	1557.367896	15.729191
28.508161	1580.267442	15.734208
28.412402	1585.364990	15.739226
28.321303	1588.302088	15.744243
28.545950	1591.813307	15.749261
28.642894	1585.463400	15.754279
28.576823	1590.903845	15.759296
28.636116	1563.200402	15.764314
28.968589	1587.092871	15.769331
28.464063	1579.427922	15.774349
28.673946	1597.960356	15.779367
28.636225	1557.995243	15.784384
28.681632	1600.332694	15.789402
28.763652	1571.269697	15.794419
28.326460	1602.459315	15.799437
29.171347	1561.699072	15.804455
29.035417	1601.935630	15.809472
28.423055	1588.606247	15.814490
28.929720	1594.796901	15.819507
28.506617	1581.364984	15.824525
28.502696	1606.564802	15.829543
28.862812	1582.448521	15.834560
28.866483	1624.320802	15.839578
28.460086	1599.051042	15.844595
29.285763	1597.198481	15.849613
28.848902	1635.233752	15.854631
29.190380	1611.183315	15.859648
28.876051	1639.967198	15.864666
29.520574	1617.364335	15.869683
29.421265	1615.588503	15.874701
29.341816	1635.173839	15.879719
29.239825	1612.962164	15.884736
29.271497	1607.508249	15.889754
29.287866	1619.115824	15.894771
29.290272	1622.478454	15.899789
29.035035	1609.505794	15.904807
29.029718	1620.895038	15.909824
29.251502	1603.021954	15.914842
29.557209	1617.244878	15.919859
29.309381	1621.219982	15.924877
29.141588	1626.432850	15.929895
29.683813	1611.826086	15.934912
29.411132	1609.355903	15.939930
29.667356	1615.253032	15.944947
29.701167	1600.433212	15.949965
29.820189	1630.459837	15.954983
29.966916	1605.032642	15.960000
29.509514	1594.563399	15.965018
29.674387	1599.218275	15.970035
30.170032	1606.189320	15.975053
29.744188	1604.253212	15.980071
29.792450	1598.164314	15.985088
29.708392	1623.507499	15.990106
29.858430	1611.439166	15.995123
29.700968	1598.546874	16.000141
29.884230	1631.691926	16.005159
30.052072	1598.773946	16.010176
29.778294	1599.190370	16.015194
29.890529	1600.298693	16.020211
29.984429	1614.487755	16.025229
29.687618	1604.477374	16.030247
29.835068	1601.230773	16.035264
29.763541	1602.686146	16.040282
29.917572	1617.644249	16.045299
30.197643	1607.011769	16.050317
30.188072	1610.146650	16.055335
30.307192	1603.274112	16.060352
29.815873	1606.215267	16.065370
29.918353	1602.505515	16.070387
29.857199	1611.519010	16.075405
29.898848	1609.324306	16.080423
30.221581	1616.129454	16.085440
30.292046	1631.525606	16.090458
30.352568	1630.136406	16.095475
30.285892	1647.517537	16.100493
30.402103	1647.502114	16.105511
30.780977	1631.724335	16.110528
30.205703	1629.563521	16.115546
30.566195	1631.835592	16.120563
30.594734	1629.904093	16.125581
30.766766	1639.640170	16.130599
30.783513	1607.800170	16.135616
30.386031	1618.014013	16.140634
30.685442	1601.355482	16.145651
30.559615	1605.457413	16.150669
30.416652	1607.345739	16.155687
30.843578	1625.338666	16.160704
30.717934	1645.087109	16.165722
30.854563	1636.187324	16.170739
30.737241	1629.852693	16.175757
30.431801	1632.913643	16.180775
30.949610	1640.607892	16.185792
30.839715	1636.494709	16.190810
31.042904	1643.123884	16.195827
30.930317	1649.215122	16.200845
30.817178	1640.216745	16.205863
31.287278	1639.347378	16.210880
30.870224	1642.463882	16.215898
30.823614	1641.692649	16.220915
31.210265	1638.631257	16.225933
30.922325	1640.901350	16.230951
30.964556	1632.925811	16.235968
30.900378	1647.745716	16.240986
30.692624	1642.451092	16.246003
30.753758	1640.133729	16.251021
31.101566	1640.800228	16.256039
31.084615	1634.292289	16.261056
30.736087	1649.959769	16.266074
30.924741	1641.861775	16.271091
31.331976	1643.140128	16.276109
31.183011	1662.697263	16.281127
31.615813	1677.916132	16.286144
31.306408	1674.729789	16.291162
31.643050	1662.916366	16.296179
31.419691	1649.411633	16.301197
31.255074	1653.482012	16.306215
31.675353	1650.924904	16.311232
31.331567	1650.830261	16.316250
31.507743	1662.863834	16.321267
31.726848	1661.306199	16.326285
31.670895	1666.114288	16.331303
31.904428	1658.622595	16.336320
31.550594	1644.349032	16.341338
31.551168	1644.363062	16.346355
31.490717	1657.212998	16.351373
31.221327	1673.025181	16.356391
31.819745	1663.944771	16.361408
31.688188	1663.250004	16.366426
31.571251	1667.355253	16.371443
31.952431	1670.138400	16.376461
31.625378	1667.964736	16.381479
31.570775	1658.477249	16.386496
31.669076	1663.550168	16.391514
31.683802	1650.698009	16.396531
32.093133	1664.729852	16.401549
31.516277	1680.883655	16.406567
32.463327	1689.944047	16.411584
32.187990	1697.613808	16.416602
32.130350	1684.153399	16.421619
32.352937	1679.771680	16.426637
32.122672	1676.728442	16.431655
31.920916	1675.816785	16.436672
31.989330	1683.296440	16.441690
32.283997	1693.432986	16.446707
32.468248	1685.883073	16.451725
31.994086	1694.668334	16.456743
32.495560	1697.721734	16.461760
32.404435	1681.092360	16.466778
32.358891	1688.505250	16.471795
32.867607	1669.562305	16.476813
32.698104	1704.308461	16.481831
32.853057	1690.924251	16.486848
32.490030	1661.175438	16.491866
32.604524	1667.441250	16.496883
32.790705	1645.943323	16.501901
32.643298	1659.461493	16.506919
32.701744	1648.969717	16.511936
32.551624	1654.348086	16.516954
32.385654	1644.541748	16.521971
32.588804	1656.135296	16.526989
32.732467	1669.657392	16.532007
32.997714	1672.918342	16.537024
32.577393	1676.076272	16.542042
32.543364	1673.391843	16.547059
32.847293	1684.197001	16.552077
32.872840	1705.175091	16.557095
33.034067	1688.409512	16.562112
33.188391	1695.579750	16.567130
32.855544	1691.156048	16.572147
32.930992	1697.778879	16.577165
32.707435	1690.696686	16.582183
32.668855	1680.207777	16.587200
32.873666	1688.058931	16.592218
32.845879	1678.367384	16.597235
33.076333	1690.244463	16.602253
33.129772	1686.113082	16.607271
33.113198	1665.556652	16.612288
33.232696	1680.166404	16.617306
33.126469	1693.769273	16.622323
33.113547	1683.605025	16.627341
33.206278	1689.768928	16.632359
33.373911	1689.024872	16.637376
33.197661	1713.168564	16.642394
33.294795	1690.608840	16.647411
33.750846	1706.140204	16.652429
33.314850	1709.767821	16.657447
33.252147	1730.928333	16.662464
33.690331	1715.952673	16.667482
33.733602	1716.202135	16.672499
33.477281	1710.981296	16.677517
33.484889	1716.263749	16.682535
33.770026	1712.667982	16.687552
33.708345	1711.452417	16.692570
33.810608	1703.174688	16.697587
34.066486	1703.484624	16.702605
33.623925	1706.032637	16.707623
33.919595	1710.978144	16.712640
34.437629	1702.428047	16.717658
33.864084	1707.424085	16.722675
33.800832	1687.763811	16.727693
34.020433	1701.385509	16.732711
34.041728	1710.431533	16.737728
33.777536	1681.609141	16.742746
34.023380	1703.247360	16.747763
34.214211	1715.133925	16.752781
33.970792	1712.415242	16.757799
33.893065	1698.759825	16.762816
34.327701	1723.465198	16.767834
34.031341	1717.654575	16.772851
34.099498	1688.774447	16.777869
33.963391	1712.122092	16.782887
33.677004	1705.904050	16.787904
33.922881	1702.989363	16.792922
33.683147	1698.363622	16.797939
34.082973	1721.907380	16.802957
34.025700	1720.138989	16.807975
34.287739	1751.541453	16.812992
34.368011	1730.030404	16.818010
34.444874	1739.412071	16.823027
34.533892	1740.178048	16.828045
34.419315	1726.003099	16.833063
34.447882	1739.955742	16.838080
34.766080	1735.274046	16.843098
34.336566	1729.074100	16.848115
34.691170	1732.934284	16.853133
34.643686	1735.935241	16.858151
34.738043	1745.762428	16.863168
34.626596	1715.819226	16.868186
34.491371	1741.504254	16.873203
34.457028	1734.395010	16.878221
34.477340	1740.029371	16.883239
34.548723	1727.087885	16.888256
34.742623	1751.476200	16.893274
34.446522	1780.798567	16.898291
34.947155	1742.263469	16.903309
34.965809	1794.514094	16.908327
34.773856	1768.942426	16.913344
34.952347	1772.575880	16.918362
35.077749	1769.667809	16.923379
35.162227	1773.637149	16.928397
34.963986	1763.717901	16.933415
35.102781	1777.269188	16.938432
35.384484	1762.955502	16.943450
35.329195	1764.306056	16.948467
35.596814	1763.981773	16.953485
35.557592	1753.238087	16.958503
35.321881	1759.662034	16.963520
35.943873	1755.318842	16.968538
35.498275	1744.081554	16.973555
35.768375	1752.249515	16.978573
35.415266	1760.139348	16.983591
35.615003	1762.210565	16.988608
35.973600	1752.674423	16.993626
35.626584	1759.907341	16.998643
36.094840	1752.057275	17.003661
35.817804	1720.638253	17.008679
35.353620	1733.887692	17.013696
35.777979	1716.592486	17.018714
35.674008	1750.049454	17.023731
35.600906	1722.034917	17.028749
35.797743	1761.578638	17.033767
35.903503	1735.753486	17.038784
35.985119	1756.310583	17.043802
36.058208	1745.685842	17.048819
36.209514	1730.482215	17.053837
35.799272	1735.504128	17.058855
35.924888	1713.896210	17.063872
35.895588	1738.348412	17.068890
35.925704	1741.379466	17.073907
36.002569	1739.734396	17.078925
36.039601	1749.437022	17.083943
36.140697	1747.830559	17.088960
35.947801	1734.710992	17.093978
35.553969	1754.072923	17.098995
36.192137	1736.248101	17.104013
36.120572	1738.980770	17.109031
35.532107	1761.672335	17.114048
36.202987	1743.285444	17.119066
36.027453	1755.313838	17.124083
36.086043	1794.832506	17.129101
35.832059	1797.090915	17.134119
36.187458	1778.925750	17.139136
36.515594	1784.918446	17.144154
36.268698	1783.785894	17.149171
36.270647	1795.192993	17.154189
36.589258	1769.064853	17.159207
36.655509	1800.652802	17.164224
36.702083	1766.496948	17.169242
36.367533	1801.392352	17.174259
37.032973	1775.328438	17.179277
37.223375	1789.098019	17.184295
36.881035	1786.789923	17.189312
36.852107	1769.024256	17.194330
37.038589	1782.605696	17.199347
36.814988	1767.002501	17.204365
37.166166	1777.288968	17.209383
36.415205	1761.958641	17.214400
36.662248	1786.687747	17.219418
37.012097	1796.537143	17.224435
36.998484	1791.095100	17.229453
37.055762	1816.677203	17.234471
37.303896	1810.353423	17.239488
37.353333	1791.461542	17.244506
37.183865	1815.122981	17.249523
37.529216	1802.386273	17.254541
37.421398	1787.766597	17.259559
37.443359	1811.730981	17.264576
37.442929	1778.963695	17.269594
37.524694	1769.894829	17.274611
37.304272	1782.551740	17.279629
37.198391	1784.599341	17.284647
37.299605	1784.040477	17.289664
37.363624	1794.509602	17.294682
37.389985	1808.130758	17.299699
37.378298	1792.419810	17.304717
37.567831	1809.955329	17.309735
37.438690	1812.942583	17.314752
37.606748	1798.086995	17.319770
37.534067	1801.285464	17.324787
37.491289	1810.629629	17.329805
37.618818	1797.152169	17.334823
37.326544	1791.265360	17.339840
37.485377	1811.212477	17.344858
37.381566	1812.573919	17.349875
37.498142	1829.167853	17.354893
37.813539	1833.639927	17.359911
37.798343	1824.471660	17.364928
37.954851	1824.665313	17.369946
37.792246	1841.602655	17.374963
38.104539	1831.177230	17.379981
38.075253	1829.880984	17.384999
37.787562	1826.848445	17.390016
38.258309	1847.090359	17.395034
38.241903	1833.627954	17.400051
38.033967	1824.915137	17.405069
38.381604	1840.570900	17.410087
38.153389	1830.730318	17.415104
38.410316	1841.714549	17.420122
38.526109	1857.045510	17.425139
38.776464	1842.459895	17.430157
38.835812	1829.380239	17.435175
38.415020	1828.321033	17.440192
38.784350	1816.011494	17.445210
38.512169	1822.556114	17.450227
38.368451	1815.775730	17.455245
38.861716	1831.304440	17.460263
38.668117	1819.241972	17.465280
38.505730	1821.146007	17.470298
38.763696	1818.306447	17.475315
38.532509	1835.018768	17.480333
38.918031	1833.705134	17.485351
38.897232	1829.349600	17.490368
39.095077	1831.844269	17.495386
39.110231	1828.145240	17.500403
38.610028	1812.642735	17.505421
39.141783	1827.435427	17.510439
38.762415	1819.967463	17.515456
38.903201	1832.958494	17.520474
39.041308	1862.260543	17.525491
38.909928	1834.335307	17.530509
38.844853	1844.384613	17.535527
39.456180	1853.775502	17.540544
39.609950	1833.619527	17.545562
39.467121	1831.616230	17.550579
39.138481	1851.419348	17.555597
39.589491	1852.568046	17.560615
39.631542	1847.318450	17.565632
39.467702	1846.521857	17.570650
39.640954	1832.376407	17.575667
39.564114	1849.224577	17.580685
40.054353	1831.366602	17.585703
39.332965	1831.233073	17.590720
39.495245	1807.984810	17.595738
39.924508	1824.933137	17.600755
39.353205	1841.196341	17.605773
39.930959	1825.503039	17.610791
39.754373	1830.541204	17.615808
39.660140	1836.988241	17.620826
39.941754	1842.426815	17.625843
40.001727	1819.824053	17.630861
39.656547	1830.382057	17.635879
39.543716	1813.554647	17.640896
39.804176	1847.367423	17.645914
40.020450	1821.942914	17.650931
39.638999	1848.255704	17.655949
40.107340	1830.498749	17.660967
40.015595	1836.851008	17.665984
40.168642	1858.221116	17.671002
39.851623	1833.462077	17.676019
39.555230	1853.409491	17.681037
40.455755	1826.468007	17.686055
39.983949	1840.214256	17.691072
39.957807	1830.478300	17.696090
40.464525	1863.611626	17.701107
40.719134	1860.962928	17.706125
40.083815	1849.254021	17.711143
40.471269	1864.620318	17.716160
40.305213	1867.179318	17.721178
40.788532	1872.061923	17.726195
40.620395	1876.548201	17.731213
40.387782	1875.814483	17.736231
40.652620	1872.369779	17.741248
40.555088	1877.689507	17.746266
41.030291	1863.016104	17.751283
40.505774	1867.191127	17.756301
40.361331	1861.505655	17.761319
40.605771	1895.091436	17.766336
40.560984	1851.123311	17.771354
40.469479	1881.615036	17.776371
40.277040	1878.818979	17.781389
40.631877	1877.448886	17.786407
41.045708	1920.236602	17.791424
40.821432	1905.644818	17.796442
40.883320	1911.994631	17.801459
40.984928	1910.842671	17.806477
41.048469	1892.635819	17.811495
41.248989	1904.560320	17.816512
41.212899	1898.870138	17.821530
41.445795	1898.493189	17.826547
40.998005	1879.521613	17.831565
41.494091	1901.818642	17.836583
41.553734	1885.842961	17.841600
41.277489	1904.660952	17.846618
41.785117	1892.319855	17.851635
41.450265	1874.972505	17.856653
41.389968	1912.083289	17.861671
41.149504	1881.589313	17.866688
41.520290	1895.264163	17.871706
41.542332	1922.782165	17.876723
41.719865	1904.604310	17.881741
42.131899	1935.418540	17.886759
41.542081	1917.238772	17.891776
41.716326	1915.068495	17.896794
42.067723	1918.918230	17.901811
41.993202	1918.774349	17.906829
42.148645	1900.988557	17.911847
42.082747	1907.382342	17.916864
41.815431	1877.141195	17.921882
41.794519	1881.531637	17.926899
42.266487	1888.918728	17.931917
42.082962	1909.365742	17.936935
42.344179	1885.684727	17.941952
41.987476	1928.395574	17.946970
42.183368	1887.302193	17.951987
42.202851	1918.698085	17.957005
41.692202	1914.104467	17.962023
42.109879	1892.264092	17.967040
42.217427	1927.443224	17.972058
42.444542	1885.599257	17.977075
42.578349	1926.323805	17.982093
42.385174	1898.908520	17.987111
42.821403	1891.842132	17.992128
42.646926	1932.883274	17.997146
42.789258	1893.308520	18.002163
42.528113	1927.223540	18.007181
42.508169	1893.392600	18.012199
42.791247	1935.826836	18.017216
42.333638	1899.871310	18.022234
42.629684	1888.352041	18.027251
42.273253	1946.576005	18.032269
42.885227	1948.886675	18.037287
42.856635	1920.808027	18.042304
42.680781	1961.484529	18.047322
43.237081	1925.637808	18.052339
43.208043	1957.041520	18.057357
43.123984	1949.296732	18.062375
43.032307	1938.391387	18.067392
43.187205	1912.856958	18.072410
43.418092	1955.960244	18.077427
42.790278	1938.983580	18.082445
43.002460	1924.666665	18.087463
43.283301	1964.365857	18.092480
43.012513	1952.858281	18.097498
43.397266	1927.000881	18.102515
42.953988	1948.963296	18.107533
43.215686	1941.707640	18.112551
43.250361	1958.662421	18.117568
43.267113	1983.170612	18.122586
43.751299	1951.227000	18.127603
43.418618	2006.542040	18.132621
43.835053	1966.987868	18.137639
43.878416	1987.930493	18.142656
43.623431	1965.953459	18.147674
43.679204	1997.497891	18.152691
43.738334	1984.750039	18.157709
44.024785	1975.522561	18.162727
43.457661	1985.427084	18.167744
43.927054	1946.493733	18.172762
44.084080	1981.444883	18.177779
43.956461	1962.513374	18.182797
44.048045	1975.328335	18.187815
44.176718	1982.178763	18.192832
44.040179	1962.061042	18.197850
43.982788	1978.841766	18.202867
43.852967	1969.372362	18.207885
44.089719	1992.565042	18.212903
44.230684	1989.368154	18.217920
44.312641	2010.644431	18.222938
44.399901	1989.580197	18.227955
44.533991	1988.223276	18.232973
44.582251	2002.973704	18.237991
44.838895	1985.001783	18.243008
44.284922	2000.703974	18.248026
44.761285	1991.645975	18.253043
44.906399	2007.892643	18.258061
45.007157	1981.079989	18.263079
44.654729	2003.825523	18.268096
44.796197	1968.013392	18.273114
44.630673	2013.863650	18.278131
44.953229	1997.715356	18.283149
44.905436	2002.402705	18.288167
44.998516	1993.349199	18.293184
44.555322	2016.401811	18.298202
44.983492	1999.503640	18.303219
45.094425	1985.452924	18.308237
44.826081	2004.540344	18.313255
44.830702	1981.271329	18.318272
44.931616	2008.128828	18.323290
45.005679	1980.107627	18.328307
45.131353	1991.504587	18.333325
45.097642	2017.737059	18.338343
45.413701	2007.759221	18.343360
45.436285	2028.332410	18.348378
45.651049	2015.009151	18.353395
45.367962	2024.578967	18.358413
45.377849	2031.309934	18.363431
45.693738	2022.815484	18.368448
45.748903	2051.607324	18.373466
45.870242	2023.016927	18.378483
45.641137	2024.305561	18.383501
45.556093	2040.102901	18.388519
46.011483	2023.621935	18.393536
45.757642	2018.282611	18.398554
45.510849	2026.769114	18.403571
46.035405	2004.730628	18.408589
45.619607	2038.952144	18.413607
45.818164	2001.178691	18.418624
46.052011	2039.804913	18.423642
46.211350	2009.997246	18.428659
46.040197	2031.295041	18.433677
46.051970	2019.240554	18.438695
46.089808	2025.278073	18.443712
45.896935	2025.577783	18.448730
45.772060	2011.061276	18.453747
46.228009	2053.768738	18.458765
45.968758	2045.598803	18.463783
46.480320	2028.550447	18.468800
46.596213	2067.020945	18.473818
46.759286	2046.257573	18.478835
46.501982	2048.614077	18.483853
46.554963	2067.238202	18.488871
46.613397	2026.142755	18.493888
46.323358	2047.467397	18.498906
46.716507	2059.136363	18.503923
46.496189	2027.504708	18.508941
46.472176	2057.421320	18.513959
47.406558	2013.557677	18.518976
46.776499	2048.961697	18.523994
46.839275	2036.817264	18.529011
46.693156	2048.361433	18.534029
46.454372	2059.412297	18.539047
47.177758	2026.492845	18.544064
46.735520	2061.561776	18.549082
46.730065	2042.532029	18.554099
47.122854	2052.297676	18.559117
47.524686	2066.741671	18.564135
47.421660	2080.378997	18.569152
47.440016	2070.602750	18.574170
47.520161	2082.375133	18.579187
47.900247	2046.457115	18.584205
47.011597	2049.746436	18.589223
47.515642	2042.867364	18.594240
47.559438	2047.228661	18.599258
47.685791	2062.501527	18.604275
47.588992	2077.729771	18.609293
47.531237	2085.258069	18.614311
47.783569	2082.406773	18.619328
47.814256	2082.126562	18.624346
47.855864	2070.200982	18.629363
48.140584	2070.960937	18.634381
47.838337	2082.597671	18.639399
48.050907	2057.903232	18.644416
48.100760	2067.791218	18.649434
47.624377	2068.828277	18.654451
48.008448	2072.204079	18.659469
48.317674	2072.588889	18.664487
48.157767	2070.715698	18.669504
48.037241	2067.985213	18.674522
47.811376	2068.033780	18.679539
47.989150	2058.079535	18.684557
47.834663	2071.275171	18.689575
47.990765	2072.102827	18.694592
48.033047	2086.111819	18.699610
47.860913	2085.612266	18.704627
48.265330	2085.116724	18.709645
48.069370	2082.736470	18.714663
48.447179	2077.224034	18.719680
48.381166	2085.011627	18.724698
48.578057	2069.372509	18.729715
49.218733	2073.572562	18.734733
49.102149	2074.670221	18.739751
49.026005	2073.304347	18.744768
48.977234	2074.570519	18.749786
48.927934	2076.639024	18.754803
49.230914	2071.789761	18.759821
49.262329	2074.082923	18.764839
49.325539	2062.507839	18.769856
49.195357	2071.955774	18.774874
48.904174	2070.501495	18.779891
48.812393	2074.450262	18.784909
49.026124	2085.979547	18.789927
49.405031	2071.456574	18.794944
49.098838	2069.465137	18.799962
48.690855	2074.678715	18.804979
49.189765	2078.039351	18.809997
49.160797	2099.536370	18.815015
49.319418	2085.523570	18.820032
49.520396	2097.998722	18.825050
49.372361	2103.866139	18.830067
49.660236	2094.948247	18.835085
49.629297	2109.629615	18.840103
49.437524	2086.199839	18.845120
49.543891	2098.675922	18.850138
49.670020	2108.164804	18.855155
49.596438	2105.367051	18.860173
49.544062	2119.446226	18.865191
49.788537	2138.305749	18.870208
49.621172	2128.128066	18.875226
49.874385	2133.747462	18.880243
49.971380	2126.120000	18.885261
49.846620	2140.827372	18.890279
49.892117	2123.010078	18.895296
50.217497	2140.584110	18.900314
50.499630	2146.496205	18.905331
50.530226	2126.752728	18.910349
50.421372	2128.387140	18.915367
50.347582	2132.029456	18.920384
50.076487	2136.892459	18.925402
50.443797	2149.746976	18.930419
50.683985	2145.698944	18.935437
50.542550	2151.365551	18.940455
50.795189	2148.056437	18.945472
51.253293	2155.672397	18.950490
51.065428	2150.821157	18.955507
51.533929	2127.982879	18.960525
51.338038	2116.914691	18.965543
51.508151	2114.899202	18.970560
51.274096	2108.968370	18.975578
51.354789	2111.338624	18.980595
51.419179	2100.428718	18.985613
51.258975	2103.900762	18.990631
51.010761	2107.172908	18.995648
51.314086	2096.906028	19.000666
51.134572	2101.457111	19.005683
51.104148	2099.427985	19.010701
50.980991	2097.004657	19.015719
51.419701	2102.149289	19.020736
51.084082	2098.177364	19.025754
51.266073	2106.343848	19.030771
51.242031	2110.574408	19.035789
50.942878	2106.486553	19.040807
51.325829	2117.701011	19.045824
51.433443	2113.587612	19.050842
51.613657	2126.898240	19.055859
51.588478	2132.851470	19.060877
51.523749	2141.142263	19.065895
51.604702	2145.568451	19.070912
51.908424	2148.180001	19.075930
51.586079	2135.121612	19.080947
51.688526	2146.188913	19.085965
51.811555	2138.322909	19.090983
51.894945	2137.832943	19.096000
52.304243	2140.987659	19.101018
51.963015	2152.861903	19.106035
51.945299	2175.686464	19.111053
52.028908	2167.513694	19.116071
52.347178	2167.687850	19.121088
52.525094	2173.456124	19.126106
52.160155	2179.595691	19.131123
52.489818	2167.410162	19.136141
52.426972	2165.496310	19.141159
52.256836	2159.511219	19.146176
52.266052	2162.358502	19.151194
52.170839	2171.503619	19.156211
52.415796	2183.515647	19.161229
52.609825	2206.526717	19.166247
52.636834	2190.993213	19.171264
52.611144	2191.593460	19.176282
52.490400	2185.510817	19.181299
52.674319	2190.760608	19.186317
53.018451	2182.384260	19.191335
52.889476	2185.096279	19.196352
53.293252	2212.550811	19.201370
53.546729	2209.205370	19.206387
53.465361	2187.569980	19.211405
53.341845	2199.164148	19.216423
53.164050	2180.276536	19.221440
53.600865	2177.276251	19.226458
53.647531	2178.519347	19.231475
53.299994	2184.019056	19.236493
53.313985	2174.731080	19.241511
53.449090	2213.510368	19.246528
53.912517	2205.723754	19.251546
54.227512	2199.840611	19.256563
54.162502	2186.500461	19.261581
54.021766	2188.651205	19.266599
53.427734	2175.548014	19.271616
54.361463	2158.477803	19.276634
53.903287	2184.578488	19.281651
53.930902	2158.324593	19.286669
54.135036	2162.355184	19.291687
53.838314	2176.627540	19.296704
53.935870	2162.026645	19.301722
53.821441	2159.852030	19.306739
54.061869	2165.251677	19.311757
53.827243	2195.713402	19.316775
54.457878	2194.337055	19.321792
54.572880	2197.412871	19.326810
54.427748	2201.322989	19.331827
54.325120	2198.421309	19.336845
54.466234	2195.015137	19.341863
54.230878	2199.625492	19.346880
54.589115	2190.712053	19.351898
54.543930	2206.147708	19.356915
54.421928	2193.390805	19.361933
54.516506	2195.555935	19.366951
54.321241	2211.710818	19.371968
54.597078	2210.022955	19.376986
54.629414	2229.301825	19.382003
54.801831	2232.379504	19.387021
55.046301	2219.405259	19.392039
54.956016	2238.234925	19.397056
55.194265	2243.263708	19.402074
54.887648	2218.614036	19.407091
54.971742	2237.889383	19.412109
55.321913	2236.299777	19.417127
54.755365	2234.230283	19.422144
55.040715	2249.986089	19.427162
55.241487	2261.563199	19.432179
55.215870	2270.629638	19.437197
55.662528	2252.726189	19.442215
55.208478	2281.146648	19.447232
55.843312	2255.039570	19.452250
55.741669	2276.373831	19.457267
55.624876	2261.849491	19.462285
55.608710	2260.272683	19.467303
55.722748	2253.782903	19.472320
55.789526	2257.635647	19.477338
55.876303	2239.764435	19.482355
56.310181	2292.691550	19.487373
56.329990	2270.912483	19.492391
55.997502	2289.132738	19.497408
56.669518	2264.284455	19.502426
56.107808	2268.352259	19.507443
56.485523	2254.441214	19.512461
56.232603	2264.829085	19.517479
56.284692	2278.685685	19.522496
56.474771	2259.906050	19.527514
56.605227	2297.158863	19.532531
56.664713	2271.626435	19.537549
56.462869	2295.295392	19.542567
56.707721	2269.494302	19.547584
56.828616	2290.601183	19.552602
56.749685	2275.071899	19.557619
56.552426	2274.639266	19.562637
56.745243	2287.246447	19.567655
56.835463	2270.285450	19.572672
57.218595	2278.800637	19.577690
57.132052	2285.831824	19.582707
57.001892	2275.630800	19.587725
57.087972	2278.420229	19.592743
57.175777	2273.696451	19.597760
57.571941	2260.018418	19.602778
57.253378	2279.189713	19.607795
57.362337	2264.468918	19.612813
57.207329	2269.860877	19.617831
57.319486	2269.899586	19.622848
57.249479	2272.706040	19.627866
57.399449	2262.012032	19.632883
57.325139	2267.661687	19.637901
57.817981	2264.339412	19.642919
57.561574	2259.176589	19.647936
57.364080	2263.999582	19.652954
57.586763	2285.269552	19.657971
57.724214	2282.516764	19.662989
57.862136	2293.754704	19.668007
57.739402	2315.185195	19.673024
57.737069	2293.873679	19.678042
58.173003	2289.781808	19.683059
57.856144	2316.173232	19.688077
58.161980	2267.817286	19.693095
58.234537	2305.801389	19.698112
57.905712	2303.761616	19.703130
58.186647	2312.739870	19.708147
58.313366	2316.446215	19.713165
58.638974	2333.708980	19.718183
59.103197	2308.815105	19.723200
58.862119	2323.306824	19.728218
58.613407	2321.185059	19.733235
58.787718	2298.119715	19.738253
58.622202	2329.232958	19.743271
58.420795	2316.700972	19.748288
58.382981	2314.839739	19.753306
58.531952	2327.718222	19.758323
58.915187	2321.382118	19.763341
58.885504	2326.806023	19.768359
58.730715	2323.284983	19.773376
59.121293	2331.556762	19.778394
59.190728	2344.864806	19.783411
59.028565	2362.318649	19.788429
59.315129	2350.518950	19.793447
59.524110	2344.767489	19.798464
59.453621	2345.851525	19.803482
59.636496	2346.571107	19.808499
59.541775	2340.259301	19.813517
59.641486	2339.554361	19.818535
59.572965	2346.233482	19.823552
59.301886	2340.014295	19.828570
59.674479	2342.454446	19.833587
59.294061	2342.611031	19.838605
59.684249	2334.320063	19.843623
59.578345	2351.079065	19.848640
59.851919	2347.934888	19.853658
60.158606	2358.337409	19.858675
60.081580	2366.874116	19.863693
60.003496	2378.240951	19.868711
59.755676	2379.664737	19.873728
59.707186	2364.570962	19.878746
60.149184	2363.555028	19.883763
60.080154	2374.681310	19.888781
60.121732	2370.158360	19.893799
60.306013	2376.100311	19.898816
60.503444	2381.725554	19.903834
60.442418	2400.328960	19.908851
60.272726	2401.005664	19.913869
60.583735	2412.212948	19.918887
60.792918	2389.003469	19.923904
60.795210	2418.274030	19.928922
60.782202	2387.403719	19.933939
60.527959	2405.908166	19.938957
61.004656	2396.434575	19.943975
61.254812	2412.848209	19.948992
61.163113	2399.504255	19.954010
61.327057	2392.152277	19.959027
61.120608	2393.380697	19.964045
61.311753	2395.051458	19.969063
61.229983	2386.270203	19.974080
61.256929	2391.663079	19.979098
61.247573	2421.427876	19.984115
61.666815	2430.392013	19.989133
61.895137	2418.621997	19.994151
61.847725	2439.879420	19.999168
61.816925	2421.262219	20.004186
62.060797	2400.636473	20.009203
61.570335	2402.096593	20.014221
61.754615	2410.494126	20.019239
61.876800	2411.273728	20.024256
61.953706	2404.689126	20.029274
62.408931	2415.501383	20.034291
62.568732	2426.682453	20.039309
62.747943	2399.876180	20.044327
62.686063	2380.561609	20.049344
62.547036	2365.405190	20.054362
62.397195	2371.535705	20.059379
62.446028	2381.754413	20.064397
62.509581	2372.118624	20.069415
62.309648	2363.471846	20.074432
62.339206	2373.485977	20.079450
62.945434	2374.844358	20.084467
62.392422	2384.072050	20.089485
62.797734	2387.191277	20.094503
62.717574	2385.770956	20.099520
62.685296	2413.505411	20.104538
62.896501	2386.011347	20.109555
62.767334	2424.535244	20.114573
63.066047	2402.917576	20.119591
62.760412	2414.735231	20.124608
62.859424	2404.063403	20.129626
63.030849	2389.055660	20.134643
62.958398	2427.419506	20.139661
63.168089	2398.544499	20.144679
63.202662	2405.860819	20.149696
63.381125	2440.232339	20.154714
63.348326	2418.515711	20.159731
63.367196	2447.175694	20.164749
63.046733	2415.290164	20.169767
63.289534	2451.430599	20.174784
63.314382	2431.820549	20.179802
63.325101	2427.492845	20.184819
63.346641	2472.936395	20.189837
63.363614	2441.977814	20.194855
63.475121	2468.740880	20.199872
63.881614	2465.174346	20.204890
63.799910	2466.091860	20.209907
63.837466	2478.692505	20.214925
64.050686	2489.811620	20.219943
64.526679	2483.872802	20.224960
64.398584	2480.333308	20.229978
64.475401	2494.715514	20.234995
64.222389	2486.839285	20.240013
64.284246	2477.324825	20.245031
64.268528	2476.290635	20.250048
64.378035	2493.833453	20.255066
64.709458	2492.505583	20.260083
64.744048	2513.275752	20.265101
64.823514	2516.293594	20.270119
64.872700	2511.272292	20.275136
64.843074	2514.157299	20.280154
65.457167	2506.068066	20.285171
65.125788	2505.418491	20.290189
65.163474	2510.470699	20.295207
65.164672	2514.440939	20.300224
65.340398	2495.371482	20.305242
65.407062	2503.081511	20.310259
65.339187	2521.030187	20.315277
65.095762	2503.525924	20.320295
65.594507	2497.431670	20.325312
65.135693	2528.117036	20.330330
65.546616	2501.916231	20.335347
65.559504	2512.681904	20.340365
65.522106	2532.244440	20.345383
65.642090	2535.139415	20.350400
65.890225	2520.318301	20.355418
65.903807	2532.483924	20.360435
65.936238	2529.568506	20.365453
66.081843	2515.699732	20.370471
66.119818	2528.892621	20.375488
65.935213	2533.774210	20.380506
66.467002	2520.505333	20.385523
66.531254	2524.519006	20.390541
66.552268	2529.098807	20.395559
66.700589	2524.595755	20.400576
66.369854	2530.318651	20.405594
66.534534	2526.762348	20.410611
66.321740	2522.886338	20.415629
66.375869	2536.110478	20.420647
66.598064	2539.764688	20.425664
66.659001	2556.152028	20.430682
66.420500	2547.114085	20.435699
66.923741	2548.919148	20.440717
66.788157	2561.623769	20.445735
67.266100	2556.423177	20.450752
67.233957	2548.416522	20.455770
67.543595	2537.219419	20.460787
67.628070	2538.775854	20.465805
67.759973	2540.770697	20.470823
67.684394	2545.883453	20.475840
67.121992	2552.152980	20.480858
67.473561	2542.369686	20.485875
67.747467	2539.973419	20.490893
67.309191	2538.304223	20.495911
67.501793	2551.261681	20.500928
67.441912	2563.225105	20.505946
67.512449	2540.560547	20.510963
67.558937	2562.911417	20.515981
67.841021	2571.406711	20.520999
68.150443	2566.667162	20.526016
68.031848	2565.882188	20.531034
67.779514	2575.348354	20.536051
67.930704	2566.499952	20.541069
68.082245	2565.699431	20.546087
68.033821	2565.203727	20.551104
68.038834	2609.959755	20.556122
68.344830	2606.734058	20.561139
68.413596	2606.360458	20.566157
68.166424	2606.777379	20.571175
68.812653	2601.487800	20.576192
68.770742	2607.054552	20.581210
68.546215	2608.698023	20.586227
68.744803	2617.490602	20.591245
68.795410	2622.573037	20.596263
69.175985	2635.019227	20.601280
69.099136	2645.731665	20.606298
69.256954	2623.167110	20.611315
69.217516	2637.240004	20.616333
69.150836	2643.573672	20.621351
69.674015	2636.018776	20.626368
69.601390	2637.880285	20.631386
69.726718	2635.134084	20.636403
69.479230	2654.408587	20.641421
69.557338	2622.725685	20.646439
70.121960	2622.228967	20.651456
69.712178	2628.840721	20.656474
69.812084	2620.499923	20.661491
70.048643	2619.554488	20.666509
69.722763	2647.315756	20.671527
70.023929	2619.554424	20.676544
69.524425	2623.639932	20.681562
69.875544	2625.576233	20.686579
69.935336	2633.897789	20.691597
69.850260	2627.665334	20.696615
70.072066	2642.945615	20.701632
70.146991	2658.975319	20.706650
70.278098	2657.278238	20.711667
70.514829	2658.524103	20.716685
70.277756	2657.113045	20.721703
70.771811	2661.832185	20.726720
70.909700	2660.889110	20.731738
70.723240	2663.668588	20.736755
71.010207	2663.550429	20.741773
70.684229	2659.597259	20.746791
70.852869	2659.852703	20.751808
70.958603	2661.062039	20.756826
71.165062	2681.217489	20.761843
71.355837	2690.825439	20.766861
71.181384	2701.145261	20.771879
71.617835	2692.662662	20.776896
71.429438	2695.925399	20.781914
71.729816	2688.969962	20.786931
71.618997	2687.428651	20.791949
71.407799	2692.150930	20.796967
71.736590	2677.683329	20.801984
71.512014	2679.391312	20.807002
71.638024	2679.291741	20.812019
71.692114	2687.677948	20.817037
71.419115	2688.004603	20.822055
71.734942	2685.825795	20.827072
71.802981	2708.614709	20.832090
71.885147	2719.800519	20.837107
72.091505	2722.955479	20.842125
71.961789	2725.536362	20.847143
72.243077	2718.097078	20.852160
71.924277	2726.546701	20.857178
72.391273	2724.481429	20.862195
72.664191	2737.077802	20.867213
72.366362	2748.062305	20.872231
72.817924	2736.298910	20.877248
72.902502	2737.704332	20.882266
72.740782	2738.532370	20.887283
73.091456	2735.029732	20.892301
73.083230	2744.700127	20.897319
73.066810	2736.152071	20.902336
73.051385	2729.770819	20.907354
73.174692	2747.248818	20.912371
73.442025	2725.419375	20.917389
72.969957	2739.382808	20.922407
73.005325	2736.921508	20.927424
73.297397	2737.655947	20.932442
73.419409	2755.870378	20.937459
73.638424	2752.105571	20.942477
73.454008	2759.136075	20.947495
74.017567	2751.697384	20.952512
73.874915	2755.493989	20.957530
73.888511	2762.736751	20.962547
74.061898	2759.482614	20.967565
74.173446	2765.367894	20.972583
74.236300	2755.575439	20.977600
74.154529	2748.006047	20.982618
74.152029	2757.579578	20.987635
74.245681	2753.816670	20.992653
73.985176	2763.390445	20.997671
74.273674	2752.386896	21.002688
74.389158	2757.209695	21.007706
74.166141	2761.451722	21.012723
74.317353	2770.962996	21.017741
74.491494	2792.301229	21.022759
74.374136	2792.085513	21.027776
74.645884	2801.560281	21.032794
74.513750	2790.644228	21.037811
74.900774	2795.795782	21.042829
74.668364	2806.915411	21.047847
75.062534	2808.593175	21.052864
75.113957	2812.443796	21.057882
75.056705	2817.968240	21.062899
75.463694	2821.057408	21.067917
75.082362	2817.625070	21.072935
75.231669	2811.643829	21.077952
75.632023	2818.660556	21.082970
75.531932	2824.141494	21.087987
75.741902	2819.382329	21.093005
75.547840	2842.247854	21.098023
75.863337	2825.879537	21.103040
75.783501	2825.180395	21.108058
75.811826	2830.941324	21.113075
75.951554	2819.867060	21.118093
76.203442	2830.025388	21.123111
76.700459	2814.360426	21.128128
77.020992	2813.649355	21.133146
76.851424	2812.879574	21.138163
76.698769	2796.289408	21.143181
76.961091	2804.120990	21.148199
76.902896	2801.269521	21.153216
77.175931	2808.801291	21.158234
76.734431	2804.615588	21.163251
77.100106	2793.104957	21.168269
76.928430	2802.882469	21.173287
77.113960	2802.069437	21.178304
77.100088	2793.333740	21.183322
76.881553	2800.582075	21.188339
76.938530	2788.665254	21.193357
76.773743	2810.064638	21.198375
77.243359	2783.222364	21.203392
77.427843	2807.278099	21.208410
77.211304	2838.461916	21.213427
77.815411	2817.405309	21.218445
77.748959	2812.357509	21.223463
77.964839	2834.187827	21.228480
78.071036	2804.067665	21.233498
77.952506	2824.004560	21.238515
78.252155	2808.372649	21.243533
77.932051	2785.687412	21.248551
77.921655	2823.157528	21.253568
78.155077	2800.026119	21.258586
77.421932	2822.284618	21.263603
78.192564	2816.074517	21.268621
77.943981	2802.670259	21.273639
78.026420	2826.930286	21.278656
78.706575	2821.782308	21.283674
78.109638	2842.316216	21.288691
78.370450	2842.637196	21.293709
78.380698	2829.218384	21.298727
78.616664	2853.704887	21.303744
78.775213	2830.050509	21.308762
78.378347	2847.689445	21.313779
78.644028	2878.622623	21.318797
79.323828	2874.018984	21.323815
78.818036	2882.673917	21.328832
79.223067	2880.170952	21.333850
79.407805	2886.688019	21.338867
79.766041	2864.401825	21.343885
79.696338	2865.503865	21.348903
80.090299	2860.168687	21.353920
80.503279	2857.881549	21.358938
79.856860	2857.786376	21.363955
79.824555	2848.793233	21.368973
79.663359	2865.972229	21.373991
79.906678	2859.712479	21.379008
80.104524	2867.205929	21.384026
79.673788	2865.077710	21.389043
79.959417	2853.536535	21.394061
80.157348	2874.381068	21.399079
79.982989	2883.316654	21.404096
80.555792	2876.620516	21.409114
80.376333	2887.154425	21.414131
80.711911	2884.496570	21.419149
80.747942	2888.386634	21.424167
80.629967	2887.872120	21.429184
80.868683	2881.237118	21.434202
80.896082	2879.823193	21.439219
80.802159	2880.855946	21.444237
81.027946	2879.105200	21.449255
80.980357	2894.495562	21.454272
81.376186	2897.364716	21.459290
81.275732	2910.743630	21.464307
81.477505	2904.936467	21.469325
81.604650	2915.386898	21.474343
81.218592	2916.637707	21.479360
81.367570	2911.164598	21.484378
81.580559	2909.197225	21.489395
81.059136	2905.983058	21.494413
81.297354	2914.810400	21.499431
81.484639	2918.700738	21.504448
81.658391	2933.291305	21.509466
81.557404	2940.122962	21.514483
81.829850	2943.660717	21.519501
82.325025	2938.171723	21.524519
82.052872	2937.182323	21.529536
82.106386	2940.320803	21.534554
82.497003	2954.769052	21.539571
82.843616	2967.262633	21.544589
82.762461	2958.753085	21.549607
82.764614	2969.855099	21.554624
82.950477	2958.745057	21.559642
83.046796	2966.882428	21.564659
83.356957	2959.851367	21.569677
82.924567	2963.890081	21.574695
83.213628	2956.964640	21.579712
83.181502	2957.502232	21.584730
83.183970	2968.128322	21.589747
82.912134	2943.371189	21.594765
83.137564	2950.745446	21.599783
83.038088	2966.317201	21.604800
83.530349	2949.318049	21.609818
83.425993	2948.998003	21.614835
83.395268	2978.051571	21.619853
83.506512	2978.283138	21.624871
83.666827	2976.471244	21.629888
83.579195	2983.900943	21.634906
83.846155	2994.532071	21.639923
84.023532	2972.996621	21.644941
84.069385	3009.802251	21.649959
84.046768	3025.346082	21.654976
84.101154	2994.075172	21.659994
83.943098	3021.193719	21.665011
84.146808	3019.812233	21.670029
84.459623	3014.891090	21.675047
84.249148	3050.350972	21.680064
84.955240	3039.043862	21.685082
84.765874	3029.038952	21.690099
84.804216	3051.489407	21.695117
84.836119	3037.125425	21.700135
84.701810	3029.488753	21.705152
84.946290	3058.251614	21.710170
84.783480	3058.257875	21.715187
84.617318	3070.695660	21.720205
85.261248	3076.366390	21.725223
85.212727	3053.949698	21.730240
85.551959	3081.314703	21.735258
85.637439	3110.780260	21.740275
86.019832	3089.909639	21.745293
86.160987	3086.493030	21.750311
86.159489	3097.001073	21.755328
86.427438	3085.306793	21.760346
86.314596	3073.329509	21.765363
85.939853	3078.249463	21.770381
86.258570	3075.423576	21.775399
86.256540	3081.834435	21.780416
86.674865	3080.057685	21.785434
86.556503	3088.698941	21.790451
86.634163	3088.345935	21.795469
86.621195	3079.465193	21.800487
86.521821	3094.878182	21.805504
86.618626	3069.192888	21.810522
86.666932	3080.224701	21.815539
86.467171	3098.221076	21.820557
87.008297	3080.738103	21.825575
86.647085	3092.115245	21.830592
86.958986	3121.679225	21.835610
87.155076	3117.141631	21.840627
87.215696	3100.937140	21.845645
87.463786	3116.885465	21.850663
87.345976	3111.208624	21.855680
87.432337	3105.024925	21.860698
87.781652	3130.604464	21.865715
87.753821	3129.535190	21.870733
88.044058	3131.875346	21.875751
87.916832	3141.689258	21.880768
88.079322	3130.461680	21.885786
88.094914	3137.135616	21.890803
88.237214	3130.762861	21.895821
88.322810	3139.221388	21.900839
87.784593	3139.350435	21.905856
88.316401	3139.669900	21.910874
88.562001	3158.167961	21.915891
88.414805	3171.276118	21.920909
88.766770	3153.625790	21.925927
88.661492	3181.658875	21.930944
88.852768	3163.585022	21.935962
89.026473	3154.977300	21.940979
89.326873	3167.659337	21.945997
89.251571	3163.754937	21.951015
88.925276	3172.467153	21.956032
89.402782	3164.376534	21.961050
89.465118	3182.339872	21.966067
89.864129	3173.076390	21.971085
90.237333	3167.372361	21.976103
89.683150	3196.582982	21.981120
89.996068	3184.172745	21.986138
90.051870	3181.398201	21.991155
89.963844	3175.936041	21.996173
90.154119	3171.639264	22.001191
90.039394	3171.088826	22.006208
89.950285	3179.524893	22.011226
90.612858	3176.599324	22.016243
90.023479	3169.666763	22.021261
90.433877	3189.723541	22.026279
90.649755	3169.920002	22.031296
90.260891	3171.703792	22.036314
90.461795	3183.168352	22.041331
90.567242	3190.966165	22.046349
90.825147	3212.887100	22.051367
90.788355	3211.914425	22.056384
90.686647	3196.542743	22.061402
90.894080	3215.272711	22.066419
90.946418	3200.589891	22.071437
91.031468	3218.456835	22.076455
91.410310	3231.179120	22.081472
90.998477	3245.700552	22.086490
91.462577	3217.486564	22.091507
91.133212	3246.775492	22.096525
92.023625	3200.148901	22.101543
91.749654	3255.810136	22.106560
91.880415	3230.158474	22.111578
92.109958	3264.416824	22.116595
92.170613	3243.259056	22.121613
92.295254	3279.582427	22.126631
92.111131	3251.809966	22.131648
92.558530	3244.004914	22.136666
92.795209	3231.910413	22.141683
92.372421	3266.699898	22.146701
92.763645	3241.057813	22.151719
92.551510	3237.343541	22.156736
92.734434	3260.122865	22.161754
92.799280	3235.066923	22.166771
92.674143	3273.575115	22.171789
93.197244	3265.056349	22.176807
93.489589	3276.476513	22.181824
93.504868	3266.467124	22.186842
93.276864	3265.959129	22.191859
93.331716	3258.498258	22.196877
93.476409	3276.697141	22.201895
93.551790	3274.899540	22.206912
93.626640	3271.456491	22.211930
93.894479	3261.177940	22.216947
93.744062	3295.091856	22.221965
93.819478	3290.790549	22.226983
94.043006	3294.948154	22.232000
94.067060	3307.186694	22.237018
94.276738	3299.237817	22.242035
94.320668	3304.647988	22.247053
94.359605	3280.855422	22.252071
94.318941	3301.679619	22.257088
94.368321	3329.473589	22.262106
95.082232	3316.209569	22.267123
95.022627	3328.963309	22.272141
95.214083	3316.758748	22.277159
95.383221	3317.533274	22.282176
95.016958	3337.754213	22.287194
95.366812	3313.522657	22.292211
95.095009	3320.541406	22.297229
95.494683	3311.522360	22.302247
95.283868	3326.637155	22.307264
95.418601	3332.967323	22.312282
95.403128	3307.043087	22.317299
95.551088	3321.521743	22.322317
95.503253	3342.181171	22.327335
95.854451	3339.202964	22.332352
95.650290	3356.490856	22.337370
96.106982	3326.044717	22.342387
95.711670	3370.665548	22.347405
95.978211	3341.523971	22.352423
96.321642	3351.542215	22.357440
96.201387	3375.295876	22.362458
96.756935	3380.144678	22.367475
96.483258	3383.870306	22.372493
96.819177	3355.019690	22.377511
96.610756	3388.564723	22.382528
96.571201	3389.323761	22.387546
97.027680	3356.753800	22.392563
96.558983	3413.282039	22.397581
96.816365	3398.020432	22.402599
97.020059	3385.662051	22.407616
96.926865	3429.696861	22.412634
96.952024	3419.425431	22.417651
97.522369	3416.568011	22.422669
97.497356	3403.873237	22.427687
97.763097	3451.940368	22.432704
97.580398	3471.025484	22.437722
97.616031	3446.111493	22.442739
97.382675	3468.409263	22.447757
98.141821	3441.786275	22.452775
98.064075	3475.896684	22.457792
97.872871	3478.451318	22.462810
98.685611	3453.975818	22.467827
98.716826	3515.425115	22.472845
98.701337	3491.975188	22.477863
99.174096	3465.391528	22.482880
98.857369	3512.273516	22.487898
98.788598	3484.983280	22.492915
99.018511	3523.605422	22.497933
99.226886	3479.646284	22.502951
99.294572	3483.384366	22.507968
98.982548	3508.432878	22.512986
99.703972	3461.759250	22.518003
99.336277	3492.712921	22.523021
98.995305	3511.367101	22.528039
99.363912	3500.412361	22.533056
99.605188	3487.498857	22.538074
99.931822	3519.304666	22.543091
99.856767	3560.367574	22.548109
99.658263	3542.109985	22.553127
100.473298	3521.528456	22.558144
100.370295	3565.713906	22.563162
100.860194	3530.330072	22.568179
100.819317	3541.669855	22.573197
100.795886	3560.896452	22.578215
101.093444	3514.191131	22.583232
100.740127	3538.060877	22.588250
101.154725	3523.617304	22.593267
100.834111	3527.354384	22.598285
100.854717	3521.531030	22.603303
101.250962	3526.315612	22.608320
100.831781	3555.600599	22.613338
101.112004	3531.482830	22.618355
101.185074	3530.743541	22.623373
101.092535	3559.072652	22.628391
101.355180	3548.107240	22.633408
101.200066	3570.740367	22.638426
101.548082	3577.509381	22.643443
101.560036	3586.021600	22.648461
101.496531	3575.264707	22.653479
101.881274	3576.642015	22.658496
101.801572	3589.199390	22.663514
102.048895	3600.224247	22.668531
102.437138	3580.368286	22.673549
102.308185	3586.649364	22.678567
102.729153	3609.138779	22.683584
102.665444	3624.428648	22.688602
102.927692	3614.069722	22.693619
102.620846	3614.099734	22.698637
102.659712	3628.412810	22.703655
103.178177	3620.851876	22.708672
103.262730	3618.649244	22.713690
103.174077	3612.897550	22.718707
103.192044	3638.040762	22.723725
103.538348	3648.636907	22.728743
103.380755	3641.928672	22.733760
103.434834	3650.353191	22.738778
103.770586	3631.587898	22.743795
103.972414	3623.297925	22.748813
103.848545	3642.712911	22.753831
104.444106	3659.304931	22.758848
104.129512	3683.326060	22.763866
104.445427	3671.329476	22.768883
104.590052	3657.782285	22.773901
104.516335	3675.977947	22.778919
104.536086	3667.775190	22.783936
104.365570	3672.064168	22.788954
104.705581	3667.685951	22.793971
105.011876	3661.687986	22.798989
104.731668	3688.765106	22.804007
105.012745	3700.138630	22.809024
105.179621	3694.553825	22.814042
105.099502	3691.804789	22.819059
105.490307	3701.175425	22.824077
105.173815	3687.617563	22.829095
105.371854	3720.619505	22.834112
105.788427	3711.786307	22.839130
106.155612	3720.174316	22.844147
105.976408	3710.657372	22.849165
105.840759	3730.757914	22.854183
106.162072	3708.137298	22.859200
106.265417	3701.980531	22.864218
106.196161	3726.898674	22.869235
106.721045	3696.149064	22.874253
106.320457	3718.073496	22.879271
106.746251	3725.917270	22.884288
106.317951	3726.090930	22.889306
106.746386	3740.964996	22.894323
106.962583	3741.556629	22.899341
106.886198	3739.276594	22.904359
106.841829	3732.616338	22.909376
106.968812	3753.158013	22.914394
107.436025	3755.860213	22.919411
107.281266	3781.622743	22.924429
107.276065	3768.323523	22.929447
107.390280	3766.536190	22.934464
107.487923	3773.921802	22.939482
107.579704	3785.288605	22.944499
107.497058	3785.139705	22.949517
107.615099	3806.973710	22.954535
107.702144	3788.742650	22.959552
107.518587	3804.204419	22.964570
108.283008	3834.643988	22.969587
108.230527	3828.015661	22.974605
108.377964	3837.182125	22.979623
109.238046	3829.332205	22.984640
108.939550	3854.685930	22.989658
109.066305	3843.706568	22.994675
109.545772	3854.821250	22.999693
109.045841	3851.966852	23.004711
109.610258	3863.075861	23.009728
109.700646	3841.006308	23.014746
109.595248	3850.814068	23.019763
109.730159	3850.768136	23.024781
109.909440	3833.752579	23.029799
109.846426	3830.824588	23.034816
109.761852	3853.207773	23.039834
109.575281	3827.877831	23.044851
109.544706	3862.830376	23.049869
109.701301	3867.928599	23.054887
109.978295	3863.441593	23.059904
110.200700	3885.278740	23.064922
110.274610	3893.080384	23.069939
110.488871	3892.936059	23.074957
110.743087	3900.898533	23.079975
110.768919	3912.902098	23.084992
110.763992	3877.122782	23.090010
110.824502	3906.453123	23.095027
111.463077	3910.632044	23.100045
111.485306	3940.353212	23.105063
111.784617	3927.798994	23.110080
111.819558	3922.323241	23.115098
111.570674	3927.660765	23.120115
112.190683	3919.524990	23.125133
112.014377	3915.409159	23.130151
112.047008	3924.465765	23.135168
112.000317	3934.804627	23.140186
112.017015	3934.904976	23.145203
112.379477	3907.573510	23.150221
112.075299	3946.429814	23.155239
112.120061	3910.139058	23.160256
112.478841	3937.418388	23.165274
112.690813	3930.940569	23.170291
112.985782	3959.293624	23.175309
113.196618	3936.151437	23.180327
113.559153	3951.618325	23.185344
113.370390	3941.858901	23.190362
113.054526	3951.836371	23.195379
113.467047	3950.404989	23.200397
113.394416	3949.787237	23.205415
113.227761	3942.079727	23.210432
113.346525	3957.924522	23.215450
113.334877	3943.359712	23.220467
113.894572	3959.200281	23.225485
113.910390	3977.795804	23.230503
113.853974	3980.804152	23.235520
113.779393	3973.332877	23.240538
114.075117	3982.157994	23.245555
114.291194	3986.626130	23.250573
114.662377	3979.188399	23.255591
114.941578	3986.082637	23.260608
114.880496	3992.481286	23.265626
114.584594	3991.821256	23.270643
114.775773	3998.467590	23.275661
114.756356	4009.157709	23.280679
115.104786	4009.227191	23.285696
114.878162	4018.827844	23.290714
114.696064	4034.516957	23.295731
115.216090	4040.598784	23.300749
115.256906	4050.738919	23.305767
115.274720	4051.601331	23.310784
116.362768	4047.783378	23.315802
116.189979	4057.944989	23.320819
116.541696	4046.911515	23.325837
116.393317	4055.637575	23.330855
116.536913	4062.056323	23.335872
116.685035	4070.200211	23.340890
116.539602	4075.687272	23.345907
116.908399	4065.744472	23.350925
117.053609	4079.526581	23.355943
116.817482	4080.229681	23.360960
117.472601	4081.453804	23.365978
117.131429	4057.436608	23.370995
117.175554	4085.855076	23.376013
117.004947	4055.933796	23.381031
117.146329	4098.806769	23.386048
117.329616	4072.059712	23.391066
117.685118	4103.103097	23.396083
117.978579	4070.013201	23.401101
117.469961	4098.659843	23.406119
117.956714	4095.104516	23.411136
118.184570	4092.768837	23.416154
118.390151	4115.603309	23.421171
118.707831	4105.888102	23.426189
118.621992	4115.471090	23.431207
118.569706	4114.669163	23.436224
118.887908	4127.456182	23.441242
118.383008	4112.460900	23.446259
118.868095	4118.790613	23.451277
119.101630	4116.434360	23.456295
118.843504	4125.946496	23.461312
119.100179	4138.789746	23.466330
119.313378	4146.407272	23.471347
119.537180	4148.991819	23.476365
119.317870	4138.918549	23.481383
119.401817	4160.941804	23.486400
119.956995	4181.214430	23.491418
119.865496	4179.758767	23.496435
119.936032	4164.485251	23.501453
120.169612	4176.773708	23.506471
120.233426	4182.719878	23.511488
120.140710	4173.298184	23.516506
120.619044	4194.774043	23.521523
120.527584	4201.838398	23.526541
120.223547	4201.226852	23.531559
120.712978	4231.632436	23.536576
121.037306	4224.111590	23.541594
120.821631	4234.270721	23.546611
120.744150	4233.638785	23.551629
121.237010	4246.593933	23.556647
121.118073	4251.158044	23.561664
121.570150	4270.740834	23.566682
121.399192	4274.441652	23.571699
122.211151	4270.984681	23.576717
122.148430	4270.055401	23.581735
122.399309	4289.239218	23.586752
122.746315	4306.208291	23.591770
122.357293	4282.341523	23.596787
122.260308	4306.355719	23.601805
122.470090	4290.962327	23.606823
122.551799	4299.216834	23.611840
122.876585	4294.688254	23.616858
122.963021	4299.458773	23.621875
122.893198	4305.611160	23.626893
122.914281	4330.943859	23.631911
122.997610	4323.260007	23.636928
123.261731	4310.125028	23.641946
123.345581	4333.525963	23.646963
123.590225	4333.964412	23.651981
124.140618	4333.319680	23.656999
123.611412	4337.957097	23.662016
124.090090	4334.413229	23.667034
124.264107	4335.209847	23.672051
123.988533	4347.849446	23.677069
124.364015	4367.040244	23.682087
124.690496	4369.757136	23.687104
125.003289	4358.888537	23.692122
124.434113	4388.529487	23.697139
124.906175	4371.721500	23.702157
125.057425	4367.784588	23.707175
124.935244	4372.354761	23.712192
124.866895	4379.949647	23.717210
124.985655	4382.332297	23.722227
125.399322	4403.742470	23.727245
125.578432	4404.180357	23.732263
125.674923	4376.555317	23.737280
125.903206	4398.112249	23.742298
125.857886	4403.915433	23.747315
126.222290	4405.572182	23.752333
126.269095	4399.288835	23.757351
126.223836	4420.935826	23.762368
126.366882	4406.139791	23.767386
126.371871	4422.758409	23.772403
126.892817	4391.965495	23.777421
126.668594	4422.417609	23.782439
126.545335	4451.911285	23.787456
126.970811	4433.369019	23.792474
127.238589	4430.640680	23.797491
127.074170	4442.811103	23.802509
127.634483	4456.580876	23.807527
127.538386	4458.404664	23.812544
127.598583	4469.836821	23.817562
127.748075	4469.794857	23.822579
127.733066	4465.222857	23.827597
127.859906	4473.757394	23.832615
127.597618	4494.452639	23.837632
128.364992	4481.374147	23.842650
128.206036	4497.523399	23.847667
128.599264	4487.393132	23.852685
128.860077	4500.128270	23.857703
128.570986	4511.166971	23.862720
128.738329	4512.276178	23.867738
128.803402	4521.224929	23.872755
128.950101	4502.123663	23.877773
129.504360	4560.632123	23.882791
129.389715	4543.969402	23.887808
129.954388	4538.890391	23.892826
129.459276	4540.873778	23.897843
129.855277	4532.677414	23.902861
129.954179	4540.635110	23.907879
129.995265	4558.956734	23.912896
130.600584	4548.691918	23.917914
130.580515	4581.211386	23.922931
130.708133	4548.112243	23.927949
131.026638	4560.487388	23.932967
131.189568	4574.418176	23.937984
131.547642	4550.135287	23.943002
131.361130	4557.765624	23.948019
131.241230	4553.965506	23.953037
131.220300	4551.009421	23.958055
131.297257	4559.116943	23.963072
131.513547	4540.013972	23.968090
131.315968	4544.796815	23.973107
131.539849	4558.326904	23.978125
131.601014	4573.199806	23.983143
131.636256	4578.309760	23.988160
132.029140	4585.878414	23.993178
132.141999	4587.405374	23.998195
132.107982	4592.017410	24.003213
132.225059	4617.801785	24.008231
132.463941	4604.929377	24.013248
132.489703	4606.012391	24.018266
132.250402	4638.453661	24.023283
132.586698	4617.748703	24.028301
133.128360	4656.137696	24.033319
133.241917	4643.121612	24.038336
133.167511	4634.141163	24.043354
133.288092	4665.652712	24.048371
133.484686	4677.622598	24.053389
133.681933	4671.439442	24.058407
133.638973	4679.793494	24.063424
134.022055	4676.477972	24.068442
133.955446	4690.011231	24.073459
134.529254	4707.901976	24.078477
134.629946	4688.633951	24.083495
134.482773	4711.439849	24.088512
134.918359	4693.556440	24.093530
134.850880	4701.053021	24.098547
134.621611	4730.549211	24.103565
135.112020	4727.682271	24.108583
134.818112	4732.512785	24.113600
135.391755	4729.816653	24.118618
135.573898	4737.941330	24.123635
135.330767	4749.204946	24.128653
135.876747	4749.192595	24.133671
135.636188	4761.464313	24.138688
135.908976	4756.076194	24.143706
135.975737	4768.603359	24.148723
136.169022	4770.881366	24.153741
136.398121	4790.005593	24.158759
136.598639	4786.229062	24.163776
136.294613	4799.029342	24.168794
137.186765	4800.494225	24.173811
136.937061	4822.938256	24.178829
137.218260	4810.942349	24.183847
137.083622	4825.786151	24.188864
136.917382	4833.340238	24.193882
137.491072	4830.588228	24.198899
137.666965	4857.995196	24.203917
137.516172	4837.238574	24.208935
137.480525	4841.866681	24.213952
137.959061	4859.458135	24.218970
138.317210	4864.514347	24.223987
138.297464	4870.796653	24.229005
138.754485	4875.627064	24.234023
138.519031	4882.607716	24.239040
138.537219	4873.099449	24.244058
138.733917	4865.308346	24.249075
138.240231	4878.566094	24.254093
138.808602	4878.976550	24.259111
139.025629	4888.200233	24.264128
139.163728	4896.857516	24.269146
139.366615	4907.888876	24.274163
139.675183	4926.770118	24.279181
139.948897	4927.349487	24.284199
139.654309	4920.933906	24.289216
139.625066	4939.152363	24.294234
140.008890	4935.965681	24.299251
140.434252	4948.313105	24.304269
140.479949	4941.264270	24.309287
140.898827	4951.178765	24.314304
141.139256	4943.340529	24.319322
141.075110	4947.008751	24.324339
140.816514	4948.585531	24.329357
141.264609	4949.788465	24.334375
141.280381	4977.046542	24.339392
141.334421	4972.070038	24.344410
141.663061	4966.676085	24.349427
141.688857	4971.388838	24.354445
141.913741	4965.038311	24.359463
142.142423	4978.680518	24.364480
142.174341	4993.735511	24.369498
142.380804	4994.452261	24.374515
142.240499	5010.518074	24.379533
142.356791	4997.048902	24.384551
142.286240	5021.453390	24.389568
142.519135	5027.487801	24.394586
142.900219	5033.371147	24.399603
143.199081	5036.318347	24.404621
143.238787	5028.539601	24.409639
143.232788	5049.547983	24.414656
143.551682	5061.381470	24.419674
143.567827	5057.422648	24.424691
143.666310	5068.484935	24.429709
143.907002	5068.839079	24.434727
144.015852	5089.942489	24.439744
144.082007	5094.813263	24.444762
144.570181	5094.161907	24.449779
144.052354	5115.762540	24.454797
144.632428	5100.933893	24.459815
144.769128	5120.303780	24.464832
144.870391	5123.476025	24.469850
145.295581	5125.075183	24.474867
145.301704	5126.491773	24.479885
145.308063	5111.611407	24.484903
145.806579	5132.080835	24.489920
145.501489	5148.913340	24.494938
145.595258	5159.764042	24.499955
145.552355	5161.894109	24.504973
145.760527	5163.708021	24.509991
145.849161	5171.303461	24.515008
146.003583	5177.311898	24.520026
146.497469	5179.051939	24.525043
146.111635	5193.155767	24.530061
146.690719	5204.362593	24.535079
146.909423	5218.423558	24.540096
146.890907	5208.125585	24.545114
147.392647	5206.554784	24.550131
147.091166	5214.234469	24.555149
147.485740	5224.221467	24.560167
147.646388	5229.382456	24.565184
147.604085	5248.995031	24.570202
148.062364	5232.351897	24.575219
147.880926	5243.295311	24.580237
148.044811	5225.159570	24.585255
148.347003	5274.578404	24.590272
148.232779	5270.737860	24.595290
148.524811	5250.947699	24.600307
148.703449	5284.029419	24.605325
148.790869	5288.563310	24.610343
148.963115	5288.415450	24.615360
148.735974	5287.676735	24.620378
149.255915	5295.323840	24.625395
149.437476	5316.622097	24.630413
149.632290	5304.352421	24.635431
149.913612	5300.792592	24.640448
149.789917	5311.299677	24.645466
150.239835	5330.634066	24.650483
150.324931	5333.786907	24.655501
150.712199	5337.692429	24.660519
150.800908	5325.561589	24.665536
150.582438	5341.106845	24.670554
150.746821	5325.901338	24.675571
150.882148	5352.267033	24.680589
151.064939	5356.990281	24.685607
151.242523	5358.568366	24.690624
151.087172	5366.763719	24.695642
151.180579	5380.621394	24.700659
151.249890	5385.619993	24.705677
151.632613	5386.607608	24.710695
151.648109	5395.894423	24.715712
151.813261	5419.989008	24.720730
152.098263	5419.444768	24.725747
152.268542	5430.866417	24.730765
152.634099	5437.022240	24.735783
153.357675	5456.193589	24.740800
153.085208	5432.154529	24.745818
153.064533	5454.555926	24.750835
153.738379	5422.781434	24.755853
153.311445	5468.468632	24.760871
153.614433	5457.846242	24.765888
153.983722	5480.423091	24.770906
154.181634	5480.637741	24.775923
153.737259	5491.439170	24.780941
153.868349	5477.633638	24.785959
154.215017	5479.308291	24.790976
154.127167	5509.070639	24.795994
154.830631	5491.286741	24.801011
154.761860	5499.499046	24.806029
155.030752	5503.755474	24.811047
155.239147	5481.956511	24.816064
155.322882	5482.271181	24.821082
155.465875	5495.803232	24.826099
155.487694	5494.284528	24.831117
155.962127	5512.066231	24.836135
155.962682	5517.015261	24.841152
155.697823	5524.358065	24.846170
155.988234	5531.572227	24.851187
155.922959	5524.676904	24.856205
156.019181	5541.632325	24.861223
156.484266	5544.151910	24.866240
156.144078	5541.777549	24.871258
156.614366	5571.974988	24.876275
156.858452	5574.581734	24.881293
156.545928	5567.077563	24.886311
157.170212	5589.577740	24.891328
157.409215	5601.114438	24.896346
157.432212	5603.942886	24.901363
157.923595	5620.578145	24.906381
157.644333	5623.986601	24.911399
158.087587	5627.709414	24.916416
158.310492	5629.303904	24.921434
158.661944	5629.878779	24.926451
158.820215	5631.304204	24.931469
158.870771	5650.011166	24.936487
159.490807	5643.403822	24.941504
159.581664	5642.741838	24.946522
159.652362	5654.229886	24.951539
159.385739	5628.671219	24.956557
159.532520	5647.508379	24.961575
159.659242	5651.365839	24.966592
159.832856	5684.728544	24.971610
159.957125	5654.289686	24.976627
159.941566	5672.617008	24.981645
160.099928	5697.206400	24.986663
160.708629	5693.067188	24.991680
160.531320	5692.821644	24.996698
160.569532	5683.635360	25.001715
160.630217	5720.105571	25.006733
160.871088	5710.426734	25.011751
161.050859	5720.975416	25.016768
161.198847	5729.401894	25.021786
161.420215	5756.633357	25.026803
161.631896	5723.738452	25.031821
161.585962	5773.374165	25.036839
162.112790	5754.725189	25.041856
162.236586	5793.677052	25.046874
162.291496	5756.738157	25.051891
162.856645	5785.491448	25.056909
162.840882	5757.529263	25.061927
162.706150	5781.062544	25.066944
163.015200	5769.870168	25.071962
163.130449	5794.795444	25.076979
163.547580	5784.171145	25.081997
163.368172	5807.947607	25.087015
163.582291	5792.211309	25.092032
163.324177	5795.440994	25.097050
163.618739	5819.691829	25.102067
163.832246	5819.598751	25.107085
164.000301	5827.058354	25.112103
164.283480	5846.486092	25.117120
163.967427	5882.315794	25.122138
164.236659	5862.786497	25.127155
164.441047	5864.247862	25.132173
164.359617	5876.918392	25.137191
164.836483	5897.195662	25.142208
165.198716	5898.632654	25.147226
165.755776	5933.530269	25.152243
165.835962	5897.538145	25.157261
165.807300	5924.682331	25.162279
166.335661	5929.487564	25.167296
166.285766	5938.523165	25.172314
166.464544	5938.324695	25.177331
166.291665	5947.298089	25.182349
166.394390	5933.567460	25.187367
166.766340	5968.113105	25.192384
166.639220	5949.449343	25.197402
166.737696	5987.530913	25.202419
167.115883	5988.101543	25.207437
167.349697	5978.097165	25.212455
167.664768	5983.552427	25.217472
167.479604	6009.910602	25.222490
167.977084	6000.200108	25.227507
168.392701	6040.947049	25.232525
168.221375	6024.262577	25.237543
168.643365	6034.505380	25.242560
168.746937	6046.473120	25.247578
168.687976	6047.170087	25.252595
168.800325	6058.102671	25.257613
168.906435	6058.867731	25.262631
169.119805	6067.579791	25.267648
169.194357	6085.500681	25.272666
169.507540	6086.464817	25.277683
170.011384	6097.782670	25.282701
170.042254	6115.665716	25.287719
170.335912	6109.425681	25.292736
170.203533	6112.214485	25.297754
170.223683	6126.718650	25.302771
170.691020	6130.809095	25.307789
170.891359	6149.458982	25.312807
171.179436	6144.320469	25.317824
170.914179	6148.539510	25.322842
171.362914	6158.744307	25.327859
171.708081	6165.217600	25.332877
171.412854	6174.372703	25.337895
171.575901	6171.040011	25.342912
171.907516	6172.293096	25.347930
171.808932	6188.872786	25.352947
172.493007	6192.026306	25.357965
172.321813	6197.207496	25.362983
172.537402	6200.114713	25.368000
172.769283	6208.995416	25.373018
172.762469	6231.243154	25.378035
173.033640	6216.160535	25.383053
172.856838	6220.027196	25.388071
173.279326	6240.577168	25.393088
173.267406	6255.842632	25.398106
173.674563	6254.247472	25.403123
173.851620	6259.125341	25.408141
174.210783	6268.929882	25.413159
174.467024	6261.756376	25.418176
174.302450	6269.167741	25.423194
174.545748	6300.001575	25.428211
175.421621	6295.874682	25.433229
175.069042	6303.614212	25.438247
175.339932	6314.718398	25.443264
175.388818	6300.402018	25.448282
175.864072	6319.506304	25.453299
176.286880	6306.473284	25.458317
176.188782	6334.576534	25.463335
176.624476	6330.228709	25.468352
176.589778	6321.139408	25.473370
176.342563	6329.892793	25.478387
176.941829	6325.446512	25.483405
176.822835	6332.473790	25.488423
176.677919	6323.586944	25.493440
176.968866	6363.176105	25.498458
176.673413	6361.618201	25.503475
177.093178	6389.993824	25.508493
177.033662	6389.071763	25.513511
177.347557	6391.440945	25.518528
177.416914	6430.732028	25.523546
177.093504	6420.022351	25.528563
177.652427	6442.367465	25.533581
178.194947	6439.287347	25.538599
178.255644	6496.606084	25.543616
178.704216	6481.342285	25.548634
178.949062	6502.485045	25.553651
179.611301	6509.346168	25.558669
179.539136	6509.191631	25.563687
179.371719	6504.957209	25.568704
179.755892	6514.912918	25.573722
179.947822	6543.872740	25.578739
180.084591	6537.445114	25.583757
180.079070	6539.337325	25.588775
180.610746	6552.702173	25.593792
180.784864	6560.820486	25.598810
180.808497	6566.371206	25.603827
181.104884	6573.203351	25.608845
181.136366	6563.183629	25.613863
181.370918	6576.627336	25.618880
181.491996	6596.428866	25.623898
181.636728	6597.562297	25.628915
182.090577	6598.849435	25.633933
182.251216	6580.788079	25.638951
182.058929	6597.059018	25.643968
182.332016	6610.990699	25.648986
182.338718	6605.401224	25.654003
182.552558	6625.700188	25.659021
182.477888	6633.018725	25.664039
182.811868	6644.221676	25.669056
182.812996	6642.172727	25.674074
182.882894	6669.611766	25.679092
183.517673	6667.824499	25.684109
183.767367	6685.315372	25.689127
183.735176	6693.273889	25.694144
184.222045	6700.960841	25.699162
184.311087	6715.341307	25.704180
184.627771	6707.377479	25.709197
184.315706	6734.643072	25.714215
184.910235	6741.111486	25.719232
184.896491	6735.837568	25.724250
184.686841	6758.786401	25.729268
185.490826	6768.019192	25.734285
185.599096	6769.211163	25.739303
185.614933	6791.481309	25.744320
185.816876	6800.379730	25.749338
185.962302	6807.827703	25.754356
186.520045	6816.077761	25.759373
186.551830	6833.809682	25.764391
186.748852	6836.673567	25.769408
187.012436	6815.958247	25.774426
187.320291	6855.725416	25.779444
187.841907	6857.395163	25.784461
187.894732	6844.474942	25.789479
187.872896	6852.687596	25.794496
188.206429	6865.818386	25.799514
188.034647	6860.821385	25.804532
188.591242	6857.330604	25.809549
188.411475	6873.017636	25.814567
188.496684	6891.983430	25.819584
188.780978	6882.822477	25.824602
188.410329	6898.260658	25.829620
188.696062	6915.130799	25.834637
189.038805	6920.442742	25.839655
189.409240	6940.217570	25.844672
189.503694	6940.270140	25.849690
189.889861	6958.290327	25.854708
189.953879	6977.474400	25.859725
190.510380	6969.234595	25.864743
190.495154	6964.978140	25.869760
190.832673	6968.399512	25.874778
190.692329	6990.584705	25.879796
191.188428	7000.271918	25.884813
191.372642	7001.701998	25.889831
191.490647	7000.418004	25.894848
191.769917	7005.013109	25.899866
191.994962	7023.078730	25.904884
192.162480	7020.370630	25.909901
191.834746	7035.780082	25.914919
191.783638	7025.788949	25.919936
192.282840	7034.461526	25.924954
192.313098	7045.924058	25.929972
192.500846	7040.774482	25.934989
193.098756	7066.709939	25.940007
193.295787	7074.483417	25.945024
193.575541	7078.350691	25.950042
193.361442	7087.168477	25.955060
193.837599	7086.611023	25.960077
193.839209	7116.948500	25.965095
194.155043	7110.307973	25.970112
194.201829	7111.447617	25.975130
194.477160	7129.378678	25.980148
194.777279	7125.700553	25.985165
194.969352	7129.949248	25.990183
194.849318	7165.513191	25.995200
195.270730	7166.953471	26.000218
195.125064	7180.023242	26.005236
195.423375	7175.405963	26.010253
195.639578	7190.934220	26.015271
195.705964	7213.895615	26.020288
196.387816	7218.157528	26.025306
196.426799	7218.855458	26.030324
196.470979	7253.383977	26.035341
196.837305	7248.753473	26.040359
196.877092	7256.818838	26.045376
197.404291	7269.715336	26.050394
197.227027	7276.684684	26.055412
197.700018	7277.266225	26.060429
198.159286	7303.548360	26.065447
197.971152	7315.946800	26.070464
198.092485	7330.481649	26.075482
198.265875	7326.246952	26.080500
198.292892	7322.997059	26.085517
198.778585	7348.497703	26.090535
199.218342	7356.509592	26.095552
199.506641	7367.075198	26.100570
199.605277	7363.256824	26.105588
199.804729	7355.110705	26.110605
199.864151	7375.133182	26.115623
199.991557	7389.056562	26.120640
200.734542	7378.007032	26.125658
200.691152	7391.889189	26.130676
200.925301	7398.639584	26.135693
201.176442	7396.819764	26.140711
200.981416	7412.293426	26.145728
201.114176	7416.880543	26.150746
201.245911	7427.925924	26.155764
201.128320	7454.873078	26.160781
201.873817	7441.254963	26.165799
201.769319	7464.310077	26.170816
202.155526	7450.434505	26.175834
201.981584	7495.293726	26.180852
202.447797	7485.317383	26.185869
202.564380	7491.110133	26.190887
202.823114	7514.589737	26.195904
203.208008	7506.388011	26.200922
203.625997	7520.417835	26.205940
203.506826	7515.409864	26.210957
203.940486	7542.497479	26.215975
203.864698	7525.730776	26.220992
204.269568	7521.614126	26.226010
204.351753	7558.673188	26.231028
204.257111	7559.431776	26.236045
204.951245	7578.275417	26.241063
204.888066	7587.790950	26.246080
205.069351	7581.421870	26.251098
205.468224	7592.530224	26.256116
205.389760	7614.165154	26.261133
205.719357	7621.061734	26.266151
205.594652	7625.663206	26.271168
206.042129	7641.639749	26.276186
206.472054	7648.639945	26.281204
206.228093	7658.511657	26.286221
206.813536	7670.314201	26.291239
206.967778	7685.294999	26.296256
207.271967	7681.627106	26.301274
207.469653	7700.708978	26.306292
207.577228	7717.703639	26.311309
207.723190	7728.056934	26.316327
207.215322	7747.687233	26.321344
207.876037	7754.627874	26.326362
208.180981	7775.579545	26.331380
208.270943	7792.273385	26.336397
208.445101	7796.710032	26.341415
208.728160	7804.208170	26.346432
208.991457	7828.154131	26.351450
209.241137	7837.158084	26.356468
209.618338	7840.641004	26.361485
209.945303	7866.264623	26.366503
210.305004	7860.690007	26.371520
210.486199	7858.148745	26.376538
210.754617	7900.103731	26.381556
210.921422	7899.738769	26.386573
211.136077	7898.026207	26.391591
211.225753	7895.527853	26.396608
211.215551	7902.057776	26.401626
211.479630	7937.095744	26.406644
211.573917	7937.426098	26.411661
212.266114	7935.956077	26.416679
212.106384	7960.492927	26.421696
212.247656	7953.425851	26.426714
212.824605	7979.367827	26.431732
212.618594	7989.379271	26.436749
212.936047	7996.303929	26.441767
213.459292	7998.117547	26.446784
213.161398	8001.357189	26.451802
213.588157	8013.190024	26.456820
213.483624	8022.792684	26.461837
214.148967	8035.036790	26.466855
214.114330	8051.600497	26.471872
214.452340	8044.557096	26.476890
214.524690	8056.046746	26.481908
214.333185	8074.745785	26.486925
214.732581	8090.012879	26.491943
214.899708	8107.569739	26.496960
215.437679	8106.712846	26.501978
215.683764	8123.637502	26.506996
215.792157	8134.495927	26.512013
216.254014	8125.060416	26.517031
216.127428	8150.898454	26.522048
216.126812	8164.985388	26.527066
216.658020	8167.022010	26.532084
216.809291	8182.844134	26.537101
216.908954	8186.075524	26.542119
217.316337	8217.471820	26.547136
217.503919	8233.484922	26.552154
217.748675	8225.439694	26.557172
217.679327	8255.335219	26.562189
218.321574	8257.214883	26.567207
218.876493	8261.371446	26.572224
219.071661	8283.069169	26.577242
219.635517	8283.504871	26.582260
219.485879	8281.696112	26.587277
219.732135	8262.796023	26.592295
219.846018	8311.962317	26.597312
220.054893	8299.399943	26.602330
220.407895	8311.378539	26.607348
220.423721	8296.872726	26.612365
220.660107	8317.467059	26.617383
220.924236	8336.512403	26.622400
220.844087	8342.284913	26.627418
221.502300	8329.812194	26.632436
221.385627	8354.118574	26.637453
221.710596	8359.503905	26.642471
221.633660	8367.767881	26.647488
221.874474	8382.882726	26.652506
222.400512	8386.654435	26.657524
222.144460	8409.892541	26.662541
222.633673	8426.520306	26.667559
222.824020	8434.677192	26.672576
222.711955	8443.411843	26.677594
223.388014	8457.896356	26.682612
223.334934	8460.686332	26.687629
224.039369	8470.216985	26.692647
224.018105	8477.555455	26.697664
224.222813	8478.677901	26.702682
224.910389	8481.860495	26.707700
224.644567	8510.079572	26.712717
225.193531	8499.989437	26.717735
225.623382	8497.384040	26.722752
225.325663	8500.316884	26.727770
225.655310	8510.897963	26.732788
225.910288	8526.647269	26.737805
226.235053	8524.997347	26.742823
226.069457	8530.179237	26.747840
226.305203	8534.581897	26.752858
226.793086	8542.207496	26.757876
226.543423	8564.341639	26.762893
226.845241	8583.965934	26.767911
227.309693	8565.751454	26.772928
227.157336	8599.948533	26.777946
227.350830	8611.935487	26.782964
227.466653	8628.730010	26.787981
228.032348	8638.703076	26.792999
227.785402	8653.035894	26.798016
228.081122	8679.450406	26.803034
228.459939	8685.476442	26.808052
228.529148	8712.780874	26.813069
228.832237	8726.805765	26.818087
229.465206	8748.963950	26.823104
229.463565	8754.790202	26.828122
230.284721	8769.107896	26.833140
230.150450	8783.258421	26.838157
230.400648	8789.087823	26.843175
231.056214	8816.282458	26.848192
230.954782	8810.122378	26.853210
231.330633	8812.066614	26.858228
231.115675	8835.589975	26.863245
231.412931	8844.967808	26.868263
231.739177	8854.591255	26.873280
231.903964	8869.594386	26.878298
232.241621	8880.334977	26.883316
232.615437	8906.226756	26.888333
232.709062	8911.265165	26.893351
232.891291	8910.885132	26.898368
233.002586	8937.002940	26.903386
233.466768	8932.726950	26.908404
233.450156	8963.690372	26.913421
233.827129	8961.492278	26.918439
233.920482	8982.894069	26.923456
233.980459	8999.651878	26.928474
234.321556	9007.643017	26.933492
234.527637	9031.251051	26.938509
234.938048	9032.381278	26.943527
235.128026	9044.805078	26.948544
235.348972	9085.154695	26.953562
236.068638	9070.481649	26.958580
236.090913	9096.513596	26.963597
236.023058	9105.731034	26.968615
236.556129	9117.340462	26.973632
236.455743	9135.355475	26.978650
236.784265	9139.097093	26.983668
236.825891	9151.759845	26.988685
237.270114	9153.205746	26.993703
237.790260	9196.676414	26.998720
237.862905	9188.109243	27.003738
238.123709	9188.935586	27.008756
238.373397	9199.242291	27.013773
238.524314	9226.686510	27.018791
238.844202	9195.662722	27.023808
238.661439	9245.237412	27.028826
238.995074	9228.968921	27.033844
239.569812	9241.270180	27.038861
239.767573	9262.772584	27.043879
240.239084	9271.969467	27.048896
240.417099	9271.856859	27.053914
241.109719	9278.572416	27.058932
240.924148	9294.357737	27.063949
241.210140	9303.657392	27.068967
241.417363	9298.557843	27.073984
241.359216	9299.197779	27.079002
241.709924	9323.332875	27.084020
241.760476	9331.064000	27.089037
241.828416	9330.854835	27.094055
242.285614	9354.387156	27.099072
242.463425	9374.221117	27.104090
242.941339	9379.866911	27.109108
242.681494	9385.479605	27.114125
242.589667	9416.288734	27.119143
243.457452	9414.077267	27.124160
243.350466	9440.859095	27.129178
243.698239	9455.951293	27.134196
243.894064	9465.672648	27.139213
244.159789	9475.014593	27.144231
244.620057	9491.453798	27.149248
244.721991	9520.728072	27.154266
245.391360	9527.122453	27.159284
245.392565	9558.087806	27.164301
245.466533	9549.975843	27.169319
246.042846	9574.659673	27.174336
246.228466	9588.806007	27.179354
246.863417	9579.869631	27.184372
246.857076	9627.176712	27.189389
247.231233	9585.128540	27.194407
247.203084	9637.255076	27.199424
247.401591	9614.697774	27.204442
247.455913	9646.170669	27.209460
248.227537	9639.999754	27.214477
247.908942	9685.527195	27.219495
248.957336	9673.549112	27.224512
248.622899	9689.084724	27.229530
248.914822	9709.059507	27.234548
249.439377	9698.066715	27.239565
249.664487	9723.559463	27.244583
249.768452	9737.493498	27.249600
249.630094	9749.218308	27.254618
250.139148	9753.127255	27.259636
250.255637	9761.583083	27.264653
250.319172	9788.917140	27.269671
250.638047	9802.420369	27.274688
251.149502	9794.107521	27.279706
251.368097	9838.067620	27.284724
251.877383	9814.637352	27.289741
251.845273	9878.901420	27.294759
252.026429	9851.965269	27.299776
252.382837	9838.057619	27.304794
252.813313	9898.455814	27.309812
252.966037	9875.330561	27.314829
253.061734	9891.978620	27.319847
253.352604	9895.156692	27.324864
253.550800	9922.170100	27.329882
253.768497	9919.637629	27.334900
254.049167	9926.001280	27.339917
254.041450	9953.305286	27.344935
254.869913	9950.658543	27.349952
254.240868	9985.491126	27.354970
255.149549	9991.384848	27.359988
255.550263	9993.808857	27.365005
255.494812	9998.944186	27.370023
255.735975	10033.266351	27.375040
255.994776	10017.547206	27.380058
256.652330	10033.342145	27.385076
256.521069	10068.665721	27.390093
256.442523	10070.750623	27.395111
257.214181	10074.426967	27.400128
257.396542	10104.579597	27.405146
257.356909	10116.427462	27.410164
257.980502	10121.102838	27.415181
258.176144	10132.362746	27.420199
258.780317	10149.285750	27.425216
258.821921	10149.724103	27.430234
258.972599	10168.979919	27.435252
259.307898	10177.267327	27.440269
259.600187	10186.906887	27.445287
260.013235	10190.300062	27.450304
260.194676	10209.582112	27.455322
260.506418	10216.750710	27.460340
260.601137	10229.979993	27.465357
260.420058	10248.738708	27.470375
260.783747	10254.514792	27.475392
261.049739	10263.505421	27.480410
261.220730	10303.531829	27.485428
261.754194	10304.889260	27.490445
261.758595	10326.105687	27.495463
262.448790	10328.080299	27.500480
262.339476	10351.006453	27.505498
262.790957	10364.907325	27.510516
263.147544	10377.772741	27.515533
263.131261	10386.148960	27.520551
263.426593	10426.782300	27.525568
263.769643	10408.616423	27.530586
263.759121	10451.217978	27.535604
264.488719	10465.915489	27.540621
264.519731	10476.268554	27.545639
264.875210	10465.048359	27.550656
265.181604	10499.972668	27.555674
265.354826	10493.674470	27.560692
265.886044	10496.005758	27.565709
266.229111	10531.825374	27.570727
266.808864	10523.215968	27.575744
266.697529	10519.743472	27.580762
267.089530	10514.559370	27.585780
267.242424	10542.746616	27.590797
267.233800	10545.653840	27.595815
267.390224	10539.037610	27.600832
267.303393	10580.666016	27.605850
267.572364	10593.754917	27.610868
267.852158	10603.946438	27.615885
268.131315	10624.923147	27.620903
268.505953	10655.873350	27.625920
268.547564	10661.214181	27.630938
268.976630	10679.655441	27.635956
269.299866	10697.669342	27.640973
269.563166	10724.266164	27.645991
269.907844	10734.340403	27.651008
270.104591	10741.500431	27.656026
270.426839	10785.562078	27.661044
271.075644	10790.180925	27.666061
271.170697	10801.691889	27.671079
271.488132	10815.002665	27.676096
272.033852	10827.311439	27.681114
272.559191	10837.365219	27.686132
272.850262	10834.169673	27.691149
272.381634	10845.511985	27.696167
273.007134	10860.908795	27.701184
273.088978	10872.797704	27.706202
273.294009	10901.779254	27.711220
273.458032	10915.570629	27.716237
273.832602	10923.329240	27.721255
274.257856	10934.072699	27.726272
274.456525	10950.604787	27.731290
274.460783	10959.767797	27.736308
275.160070	10979.981556	27.741325
274.997717	10992.429681	27.746343
275.557279	11004.653762	27.751360
275.896062	11017.548538	27.756378
275.604336	11036.999534	27.761396
276.293422	11045.677267	27.766413
276.486807	11083.721315	27.771431
276.857438	11085.187411	27.776448
277.352291	11112.004184	27.781466
277.320307	11122.074969	27.786484
277.699242	11140.419328	27.791501
277.862704	11152.616547	27.796519
278.240834	11172.184468	27.801536
278.937820	11177.505241	27.806554
279.136328	11191.837554	27.811572
279.634320	11197.957378	27.816589
279.610071	11199.989710	27.821607
279.807414	11207.496147	27.826624
280.450504	11203.662432	27.831642
280.724568	11222.580018	27.836660
281.018301	11232.562765	27.841677
281.377962	11223.665764	27.846695
281.360584	11221.423566	27.851712
281.859988	11247.510696	27.856730
281.377932	11266.874270	27.861748
282.035735	11248.124812	27.866765
282.382796	11270.597538	27.871783
282.396308	11286.606239	27.876800
282.740119	11296.820298	27.881818
282.764139	11328.822940	27.886836
283.099499	11334.657870	27.891853
282.997339	11363.905696	27.896871
283.479286	11379.629707	27.901888
283.723421	11391.123659	27.906906
283.988168	11406.984036	27.911924
284.140036	11419.575647	27.916941
284.778828	11435.788248	27.921959
284.741477	11463.808030	27.926976
285.282001	11479.165898	27.931994
285.965595	11502.382193	27.937012
286.124748	11510.075882	27.942029
286.567409	11522.740469	27.947047
286.822788	11529.483066	27.952064
287.456606	11532.385290	27.957082
287.582879	11561.669105	27.962100
287.704133	11555.594787	27.967117
288.103560	11572.398961	27.972135
288.246389	11576.599724	27.977152
288.582160	11591.653886	27.982170
288.569355	11615.623947	27.987188
288.770045	11626.674038	27.992205
289.304277	11649.136389	27.997223
289.539021	11652.781443	28.002240
289.810300	11663.674711	28.007258
289.961937	11693.812207	28.012276
290.397704	11709.577373	28.017293
290.559454	11719.483099	28.022311
290.826350	11748.068412	28.027328
291.286946	11751.995458	28.032346
291.692874	11788.427444	28.037364
292.198556	11779.288053	28.042381
292.167857	11788.633826	28.047399
292.352915	11823.377491	28.052416
293.336346	11813.399303	28.057434
293.220880	11835.791147	28.062452
293.732738	11844.309099	28.067469
294.276709	11852.046312	28.072487
294.090298	11864.086187	28.077504
294.530667	11874.127450	28.082522
294.350817	11898.320161	28.087540
295.013925	11885.134630	28.092557
295.050299	11887.375796	28.097575
295.152997	11937.661544	28.102592
295.702574	11919.730111	28.107610
295.809168	11932.197142	28.112628
295.791152	11946.877531	28.117645
296.072494	11979.370223	28.122663
296.394681	11995.397774	28.127680
296.653996	12008.481972	28.132698
296.618511	12033.671509	28.137716
297.013311	12051.391112	28.142733
297.446096	12070.484379	28.147751
297.661616	12093.459004	28.152768
298.165219	12123.104058	28.157786
298.229626	12152.845531	28.162804
298.528165	12156.837077	28.167821
298.989373	12183.203057	28.172839
299.028254	12204.973080	28.177856
299.879864	12219.254628	28.182874
299.869760	12267.366904	28.187892
300.207163	12267.721779	28.192909
300.797394	12287.661111	28.197927
301.005973	12301.520639	28.202944
301.712506	12317.117363	28.207962
301.952490	12337.410284	28.212980
301.935969	12354.735165	28.217997
302.450846	12363.642136	28.223015
302.478667	12386.212856	28.228032
303.071050	12404.135144	28.233050
303.417942	12415.905702	28.238068
303.868351	12436.565250	28.243085
303.925069	12459.548619	28.248103
304.418158	12468.333391	28.253120
305.078227	12465.968683	28.258138
305.003346	12491.919470	28.263156
305.063863	12503.008874	28.268173
305.479766	12508.438484	28.273191
305.618264	12522.912280	28.278208
306.181328	12538.630483	28.283226
306.145070	12558.851041	28.288244
306.792705	12570.428381	28.293261
307.159537	12593.742494	28.298279
307.307739	12611.932585	28.303296
307.779345	12616.457270	28.308314
307.712509	12643.720667	28.313332
307.967666	12650.864034	28.318349
308.554524	12669.831384	28.323367
308.653090	12682.202912	28.328384
309.313160	12695.829500	28.333402
309.599959	12725.013640	28.338420
310.023223	12731.590316	28.343437
310.157028	12744.590078	28.348455
310.147130	12761.700282	28.353472
310.869636	12778.956675	28.358490
311.191905	12804.739039	28.363508
310.878109	12817.000085	28.368525
311.512565	12838.759735	28.373543
311.535230	12849.503005	28.378560
311.919924	12861.735812	28.383578
312.224112	12863.356129	28.388596
312.662371	12893.878910	28.393613
313.208389	12896.182259	28.398631
313.168172	12923.627473	28.403648
313.963750	12918.591750	28.408666
314.239685	12929.875787	28.413684
314.169541	12946.188635	28.418701
314.715332	12959.897233	28.423719
314.768039	12970.549221	28.428736
315.068930	12983.313588	28.433754
315.221432	12996.231484	28.438772
315.263973	13021.058985	28.443789
316.266986	13049.203789	28.448807
316.059714	13085.437326	28.453824
316.843165	13086.524774	28.458842
316.948944	13108.849786	28.463860
317.050753	13145.785305	28.468877
317.459255	13144.070202	28.473895
318.007715	13173.400642	28.478912
318.408448	13171.183616	28.483930
318.498954	13216.651770	28.488948
318.990172	13222.218992	28.493965
319.845964	13235.277286	28.498983
319.744674	13245.982147	28.504000
320.405531	13251.137253	28.509018
320.664768	13274.237365	28.514036
320.700480	13286.088692	28.519053
321.093044	13292.578809	28.524071
321.264285	13311.494148	28.529088
321.881156	13336.650370	28.534106
321.720505	13348.890191	28.539124
322.112602	13359.775665	28.544141
322.272873	13383.036346	28.549159
322.603614	13410.762965	28.554176
323.166844	13425.117007	28.559194
323.477261	13435.755606	28.564212
323.558660	13463.105276	28.569229
323.958687	13475.491791	28.574247
324.418332	13506.826481	28.579264
324.407352	13518.210992	28.584282
324.880178	13541.855419	28.589300
325.275299	13559.225881	28.594317
325.737705	13581.472717	28.599335
325.660725	13605.678512	28.604352
326.242337	13624.126033	28.609370
326.623922	13654.643833	28.614388
326.720644	13672.288275	28.619405
327.208609	13682.830668	28.624423
327.273736	13716.422988	28.629440
327.949465	13724.888743	28.634458
328.241625	13754.613984	28.639476
328.309152	13788.253702	28.644493
328.890780	13789.503643	28.649511
329.099732	13810.237392	28.654528
329.608904	13819.360044	28.659546
330.254638	13832.771518	28.664564
330.379631	13855.472982	28.669581
330.726577	13867.277134	28.674599
330.907955	13886.816958	28.679616
331.770834	13883.120352	28.684634
331.932485	13900.625917	28.689652
332.018810	13908.243685	28.694669
332.627273	13910.610156	28.699687
332.369971	13935.427795	28.704704
332.891479	13945.526980	28.709722
333.189157	13966.909288	28.714740
333.851246	13972.759404	28.719757
334.145314	13988.561735	28.724775
334.076042	14005.995101	28.729792
334.925688	14028.520640	28.734810
335.023703	14029.480363	28.739828
335.004306	14051.161661	28.744845
335.503711	14064.066611	28.749863
335.566905	14100.595181	28.754880
335.906319	14117.692375	28.759898
336.322721	14128.657674	28.764916
336.823012	14159.876738	28.769933
336.921660	14168.475636	28.774951
337.128860	14217.671906	28.779968
337.680314	14214.353982	28.784986
338.245065	14241.239957	28.790004
338.446265	14277.426683	28.795021
338.761015	14275.418423	28.800039
339.066318	14302.460996	28.805056
339.235363	14339.478335	28.810074
339.746081	14343.864974	28.815092
340.021921	14377.485195	28.820109
340.479713	14394.527036	28.825127
340.804887	14425.852579	28.830144
341.090533	14422.513798	28.835162
341.835612	14457.412668	28.840180
342.026488	14467.498767	28.845197
342.287458	14481.904734	28.850215
342.728351	14498.774632	28.855232
342.634514	14527.633139	28.860250
343.270471	14547.364587	28.865268
343.575906	14568.083207	28.870285
344.033241	14590.749339	28.875303
344.124223	14617.113610	28.880320
344.633601	14633.384032	28.885338
345.097305	14651.317687	28.890356
345.353515	14665.576497	28.895373
345.883294	14686.557282	28.900391
346.502972	14702.733453	28.905408
346.868562	14717.055666	28.910426
346.980585	14728.735076	28.915444
347.504767	14749.609882	28.920461
348.091607	14756.604569	28.925479
348.016885	14781.057962	28.930496
348.091061	14764.118690	28.935514
348.636360	14797.215534	28.940532
348.387277	14816.903469	28.945549
349.273404	14821.143838	28.950567
349.460547	14844.271401	28.955584
349.637754	14862.806912	28.960602
350.141628	14878.853830	28.965620
350.119537	14902.158877	28.970637
350.826618	14924.711026	28.975655
350.680541	14965.168485	28.980672
351.177885	14969.009844	28.985690
351.742248	14976.928058	28.990708
351.804748	15012.068823	28.995725
352.335349	15035.529545	29.000743
352.890353	15047.810094	29.005760
352.821653	15075.416631	29.010778
353.392740	15103.861294	29.015796
353.558760	15119.704368	29.020813
354.105623	15149.240699	29.025831
354.480724	15171.293197	29.030848
354.893029	15184.874728	29.035866
355.467662	15214.102011	29.040884
355.668391	15236.310014	29.045901
356.042129	15256.751133	29.050919
356.146514	15278.788472	29.055936
356.603770	15305.328286	29.060954
357.233442	15327.320470	29.065972
357.717825	15325.047998	29.070989
357.885026	15367.358615	29.076007
358.278882	15372.065191	29.081024
358.372471	15409.234711	29.086042
358.919097	15433.021566	29.091060
358.952000	15447.920686	29.096077
359.240285	15461.522620	29.101095
360.020308	15501.365922	29.106112
359.718456	15500.264535	29.111130
360.527877	15547.155247	29.116148
360.834960	15578.951880	29.121165
361.673738	15580.143692	29.126183
361.763792	15605.479328	29.131200
361.992104	15646.094628	29.136218
362.765981	15648.603596	29.141236
362.986405	15663.097929	29.146253
363.286511	15679.685434	29.151271
363.814490	15692.454667	29.156288
364.244176	15735.017720	29.161306
364.456744	15744.224716	29.166324
365.304834	15757.135280	29.171341
365.216133	15763.454183	29.176359
365.432510	15806.194995	29.181376
365.919107	15819.038040	29.186394
366.538112	15822.871355	29.191412
366.641755	15842.362794	29.196429
366.553609	15888.370511	29.201447
367.313864	15885.767938	29.206464
367.154827	15934.785711	29.211482
367.814099	15932.888260	29.216500
368.049675	15956.375068	29.221517
368.564523	15982.928236	29.226535
369.117845	16001.550446	29.231552
369.167390	16010.891825	29.236570
369.779590	16029.973103	29.241588
370.087324	16059.591020	29.246605
370.106905	16073.800972	29.251623
370.929355	16105.965219	29.256640
371.066736	16095.225280	29.261658
371.332487	16150.382002	29.266676
371.333123	16151.534315	29.271693
371.790290	16209.003140	29.276711
372.363832	16200.695651	29.281728
372.304819	16260.287792	29.286746
373.191754	16259.871878	29.291764
373.329896	16321.680190	29.296781
373.909109	16320.759068	29.301799
374.294026	16341.541826	29.306816
374.560581	16388.123155	29.311834
375.240268	16399.573156	29.316852
375.205100	16431.635306	29.321869
375.966971	16462.283528	29.326887
376.325669	16485.952678	29.331904
376.562322	16513.972914	29.336922
377.509334	16515.930319	29.341940
377.784643	16548.030630	29.346957
377.891172	16568.078250	29.351975
378.404802	16576.884780	29.356992
378.833866	16604.502337	29.362010
379.259658	16639.535503	29.367028
379.865145	16643.066998	29.372045
379.707670	16667.587848	29.377063
380.566130	16678.454736	29.382080
380.548510	16722.007311	29.387098
381.260520	16714.011889	29.392116
381.442216	16767.582379	29.397133
381.455073	16766.185805	29.402151
381.913476	16802.187435	29.407168
382.600221	16807.915953	29.412186
383.076209	16866.415984	29.417204
383.273891	16872.428329	29.422221
383.739320	16887.967217	29.427239
384.341011	16910.795459	29.432256
384.103217	16936.619325	29.437274
385.101153	16932.750138	29.442292
385.168115	16977.133548	29.447309
385.507734	17006.411146	29.452327
386.042913	17009.640584	29.457344
386.229891	17045.391971	29.462362
386.816389	17066.688604	29.467380
387.066270	17085.755513	29.472397
387.597240	17111.342237	29.477415
388.160346	17120.181155	29.482432
388.404495	17147.936815	29.487450
388.952394	17140.511751	29.492468
389.312621	17180.347969	29.497485
389.324209	17188.246569	29.502503
389.578828	17197.684622	29.507520
389.583355	17231.022869	29.512538
390.194441	17248.257624	29.517556
390.858921	17281.646721	29.522573
390.957317	17310.350207	29.527591
391.417664	17323.804739	29.532608
391.430245	17362.138907	29.537626
391.924901	17396.094035	29.542644
392.367883	17384.266327	29.547661
392.613297	17446.972990	29.552679
393.647681	17462.919598	29.557696
393.776658	17488.288938	29.562714
394.265773	17517.140182	29.567732
394.854016	17544.449839	29.572749
394.995117	17555.137188	29.577767
395.495105	17603.146972	29.582784
395.571393	17613.756705	29.587802
396.136126	17630.013335	29.592820
396.714671	17684.315245	29.597837
397.022366	17678.469609	29.602855
397.525628	17737.503593	29.607872
397.514002	17747.407008	29.612890
398.277032	17755.619803	29.617908
398.910561	17805.256845	29.622925
399.120783	17832.849469	29.627943
399.626646	17832.670812	29.632960
399.826144	17891.257950	29.637978
400.206978	17882.721829	29.642996
400.768914	17943.789240	29.648013
401.086764	17936.087088	29.653031
401.488994	17987.282727	29.658048
402.231170	17995.185412	29.663066
402.506589	18011.234618	29.668084
402.835302	18044.824328	29.673101
403.041052	18079.204131	29.678119
403.773041	18075.527435	29.683136
403.945111	18125.309888	29.688154
404.184010	18146.325030	29.693172
404.920690	18149.066140	29.698189
404.742294	18200.328614	29.703207
405.527697	18214.026022	29.708224
405.820182	18227.572064	29.713242
406.514782	18267.054872	29.718260
406.796494	18282.182531	29.723277
406.823440	18323.332417	29.728295
407.883937	18324.462583	29.733312
408.406156	18357.300910	29.738330
408.402128	18397.465021	29.743348
409.239583	18403.591186	29.748365
409.213311	18430.770798	29.753383
409.833855	18455.935262	29.758400
409.775789	18480.911828	29.763418
410.332047	18499.047444	29.768436
410.624556	18515.031854	29.773453
410.799996	18532.694338	29.778471
411.556493	18557.070791	29.783488
411.430006	18593.564065	29.788506
411.879558	18624.716150	29.793524
412.644694	18643.386362	29.798541
412.748622	18663.737502	29.803559
413.377129	18714.953825	29.808576
413.684042	18711.582107	29.813594
414.227439	18766.432579	29.818612
414.557569	18779.492798	29.823629
414.755596	18809.632976	29.828647
415.453466	18840.551053	29.833664
415.895028	18865.400606	29.838682
416.038541	18900.732692	29.843700
416.637541	18904.526979	29.848717
417.263934	18988.467334	29.853735
417.574065	18969.175717	29.858752
417.931928	19029.926375	29.863770
418.281911	19036.267076	29.868788
418.890541	19068.494716	29.873805
419.325464	19115.709312	29.878823
419.608868	19118.489748	29.883840
420.165222	19166.036730	29.888858
420.394775	19191.431220	29.893876
421.198131	19208.793251	29.898893
421.403819	19242.087826	29.903911
421.851796	19267.081885	29.908928
422.115982	19292.843471	29.913946
422.686726	19323.520555	29.918964
423.209912	19352.531610	29.923981
423.760681	19383.990756	29.928999
423.958188	19403.883062	29.934016
424.385080	19432.574164	29.939034
424.457979	19469.236548	29.944052
425.424449	19486.486683	29.949069
425.548800	19525.063904	29.954087
426.346782	19549.389249	29.959104
426.311996	19578.407331	29.964122
426.699003	19609.788689	29.969140
427.552849	19621.983867	29.974157
427.552496	19670.101416	29.979175
428.532265	19686.898849	29.984192
429.027546	19727.506553	29.989210
429.397320	19750.603517	29.994228
429.998093	19771.470684	29.999245
430.183493	19798.662664	30.004263
430.659503	19815.637347	30.009280
431.309163	19841.089598	30.014298
431.665282	19867.682026	30.019316
431.996282	19879.494141	30.024333
432.007450	19913.843643	30.029351
432.901167	19925.898057	30.034368
433.200862	19948.280055	30.039386
433.174529	19986.607995	30.044404
433.917683	19996.997755	30.049421
434.336566	20019.444338	30.054439
434.662421	20045.206794	30.059456
435.404472	20062.195274	30.064474
435.511233	20089.346347	30.069492
435.772321	20111.246505	30.074509
436.121454	20137.382993	30.079527
436.214425	20168.224478	30.084544
436.973837	20204.394152	30.089562
437.262402	20232.594551	30.094580
437.985108	20265.399463	30.099597
438.329655	20292.350002	30.104615
438.600000	20319.895924	30.109632
439.559072	20346.061195	30.114650
439.773805	20371.845043	30.119668
440.928799	20408.411663	30.124685
440.435764	20431.237995	30.129703
441.263567	20443.705717	30.134720
441.878498	20470.243375	30.139738
441.851185	20505.140122	30.144756
442.381336	20542.155845	30.149773
442.894131	20574.747580	30.154791
443.293848	20583.264294	30.159808
443.492601	20639.415374	30.164826
443.769956	20662.503213	30.169844
444.526186	20693.731466	30.174861
444.708496	20739.159914	30.179879
444.950541	20776.422900	30.184896
445.844713	20805.132257	30.189914
445.874730	20863.775883	30.194932
446.461824	20887.053716	30.199949
447.027954	20907.685377	30.204967
447.565102	20958.714553	30.209984
448.237495	20991.641621	30.215002
448.383030	21011.683643	30.220020
449.119633	21066.547263	30.225037
449.667330	21089.316643	30.230055
449.800767	21120.316572	30.235072
450.692564	21162.508378	30.240090
451.035336	21183.600850	30.245108
451.467791	21207.693279	30.250125
452.017651	21249.324742	30.255143
452.519655	21277.431991	30.260160
452.881511	21313.863267	30.265178
452.881409	21328.426092	30.270196
453.760794	21369.792356	30.275213
454.385009	21398.335937	30.280231
454.761589	21423.527928	30.285248
455.684947	21435.162201	30.290266
455.533915	21473.147439	30.295284
455.684871	21510.798787	30.300301
456.617999	21534.681626	30.305319
456.859351	21559.513425	30.310336
457.193015	21578.452401	30.315354
457.436952	21610.429956	30.320372
458.082181	21637.890915	30.325389
458.443180	21647.375963	30.330407
458.625212	21711.695979	30.335424
459.492367	21717.573045	30.340442
459.743693	21743.280867	30.345460
459.750809	21792.385411	30.350477
460.530156	21805.943251	30.355495
461.428615	21844.304820	30.360512
461.529253	21875.856053	30.365530
461.743649	21920.649224	30.370548
462.285019	21943.255470	30.375565
462.802115	21975.601357	30.380583
463.346342	22013.553536	30.385600
463.726517	22046.861723	30.390618
464.156178	22081.401715	30.395636
464.603063	22098.451255	30.400653
465.229131	22157.457208	30.405671
465.751138	22187.299873	30.410688
466.251694	22221.375242	30.415706
466.332801	22256.710667	30.420724
467.122062	22293.415573	30.425741
467.517130	22326.302203	30.430759
468.001191	22376.776211	30.435776
468.757866	22407.553779	30.440794
469.150638	22441.468803	30.445812
469.666273	22478.531183	30.450829
470.166596	22516.671926	30.455847
470.204277	22532.993241	30.460864
471.215438	22572.794877	30.465882
471.281039	22604.587849	30.470900
472.140136	22637.557155	30.475917
472.731346	22685.516858	30.480935
473.151287	22693.036779	30.485952
473.278450	22747.107466	30.490970
474.218951	22768.621939	30.495988
474.623344	22791.103159	30.501005
475.110846	22830.259550	30.506023
475.328731	22857.512695	30.511040
476.033515	22893.223544	30.516058
476.174621	22928.632039	30.521076
476.985322	22947.699091	30.526093
477.378274	23002.279635	30.531111
477.883047	23025.119311	30.536128
478.594859	23042.827858	30.541146
478.723412	23092.343984	30.546164
479.284483	23117.175355	30.551181
479.737578	23148.255555	30.556199
479.758648	23189.749947	30.561216
480.443917	23218.186297	30.566234
480.407602	23256.886881	30.571252
481.228692	23293.445703	30.576269
481.720593	23334.584296	30.581287
481.978074	23363.329274	30.586304
482.833872	23408.784555	30.591322
483.419630	23415.909016	30.596340
483.418806	23491.808071	30.601357
484.029498	23488.203444	30.606375
484.373401	23563.045276	30.611392
485.144351	23558.822019	30.616410
485.339746	23627.556090	30.621428
486.004386	23629.513005	30.626445
486.568734	23686.311008	30.631463
486.937911	23701.971091	30.636480
488.069096	23743.307433	30.641498
488.216577	23783.833348	30.646516
488.365928	23822.756209	30.651533
488.944658	23827.045664	30.656551
489.522081	23868.970698	30.661568
490.363623	23894.304458	30.666586
490.506418	23919.806270	30.671604
490.701343	23974.513075	30.676621
491.368264	24000.104814	30.681639
491.659787	24040.005096	30.686656
492.192458	24085.825706	30.691674
492.719998	24130.817071	30.696692
493.067249	24157.595003	30.701709
493.414104	24223.088350	30.706727
494.191453	24243.676969	30.711744
495.011986	24282.448363	30.716762
495.609581	24331.968476	30.721780
496.029691	24363.937721	30.726797
496.944087	24394.526273	30.731815
497.147681	24433.657025	30.736832
497.554239	24460.348830	30.741850
498.118721	24488.747631	30.746868
498.977686	24527.114937	30.751885
499.373594	24567.493006	30.756903
499.498369	24594.493793	30.761920
499.876429	24631.179839	30.766938
500.439511	24682.617469	30.771956
500.853726	24702.643042	30.776973
501.543933	24752.053615	30.781991
501.896968	24794.695826	30.787008
502.648344	24827.667175	30.792026
503.057743	24858.689161	30.797044
503.586767	24908.882084	30.802061
504.217773	24918.910576	30.807079
504.734607	24962.988333	30.812096
505.453633	25004.424341	30.817114
505.986323	25006.042475	30.822132
506.512853	25073.558736	30.827149
507.360591	25066.314611	30.832167
507.351098	25116.015785	30.837184
507.952120	25132.154731	30.842202
508.701336	25165.995185	30.847220
508.831041	25212.593745	30.852237
509.414490	25216.021076	30.857255
509.697122	25274.379679	30.862272
510.808024	25285.278017	30.867290
511.060816	25319.993464	30.872308
511.285971	25346.169761	30.877325
511.739065	25360.215893	30.882343
511.841011	25394.776717	30.887360
512.328258	25433.317277	30.892378
512.899461	25474.997832	30.897396
513.043060	25522.687662	30.902413
513.863666	25552.927883	30.907431
513.852616	25593.923209	30.912448
514.258539	25640.105635	30.917466
515.181248	25690.271400	30.922484
515.423731	25733.242523	30.927501
516.209654	25763.182238	30.932519
516.611543	25830.244968	30.937536
517.413664	25857.787535	30.942554
517.779677	25895.595435	30.947572
518.539824	25946.166017	30.952589
518.996962	25972.571075	30.957607
519.601384	26034.061353	30.962624
520.291833	26059.901600	30.967642
520.922055	26116.743476	30.972660
521.046880	26130.177704	30.977677
521.851276	26176.452615	30.982695
522.351817	26187.532300	30.987712
522.594455	26263.495571	30.992730
523.434177	26271.018883	30.997748
523.427616	26344.565185	31.002765
524.433153	26368.949577	31.007783
524.687656	26418.333087	31.012800
525.373411	26457.477084	31.017818
525.992505	26518.922773	31.022836
526.527648	26541.549976	31.027853
527.663856	26575.819424	31.032871
528.176223	26610.830349	31.037888
528.401890	26664.566200	31.042906
528.841406	26685.750647	31.047924
529.343403	26715.575087	31.052941
530.059137	26735.160511	31.057959
530.400030	26798.789643	31.062976
530.675844	26799.917914	31.067994
531.312810	26876.138762	31.073012
531.328948	26923.907419	31.078029
532.356245	26940.014184	31.083047
532.597394	27005.969063	31.088064
533.570919	27045.761145	31.093082
533.828382	27082.083638	31.098100
534.151113	27135.121787	31.103117
534.897723	27176.840288	31.108135
535.389374	27224.837412	31.113152
535.961442	27256.763039	31.118170
536.684488	27298.534455	31.123188
536.548718	27347.710394	31.128205
537.593104	27378.576265	31.133223
538.296373	27415.890493	31.138240
538.740198	27455.198359	31.143258
539.518980	27490.030903	31.148276
539.804377	27511.105480	31.153293
540.742179	27539.923742	31.158311
540.730825	27586.303497	31.163328
541.149327	27622.175345	31.168346
541.935082	27655.075371	31.173364
542.234672	27701.391753	31.178381
542.712226	27740.045765	31.183399
543.550625	27781.752796	31.188416
543.984063	27819.608852	31.193434
544.767697	27849.598536	31.198452
545.331951	27897.118123	31.203469
545.795909	27940.401016	31.208487
546.112014	27978.930048	31.213504
546.541015	28019.833111	31.218522
547.455480	28044.725403	31.223540
547.573659	28094.103466	31.228557
548.624907	28133.160252	31.233575
549.291443	28170.874437	31.238592
549.278184	28221.373674	31.243610
550.051700	28259.364113	31.248628
550.695245	28306.095443	31.253645
551.403985	28341.382981	31.258663
551.801418	28389.554579	31.263680
552.125165	28425.139975	31.268698
553.737237	28463.251042	31.273716
553.636723	28500.809252	31.278733
554.223193	28533.182634	31.283751
554.614764	28564.417907	31.288768
554.845644	28607.875226	31.293786
555.683261	28649.661843	31.298804
556.167216	28693.457271	31.303821
556.744384	28725.181726	31.308839
557.052752	28790.238940	31.313856
557.403651	28831.449593	31.318874
558.312306	28876.336080	31.323892
558.500966	28919.811990	31.328909
559.237255	28974.931036	31.333927
560.085160	29017.166068	31.338944
560.337892	29071.815651	31.343962
560.744976	29104.179350	31.348980
561.637786	29158.350669	31.353997
562.082416	29203.950171	31.359015
562.033896	29259.901139	31.364032
562.427987	29324.261359	31.369050
563.800471	29354.082852	31.374068
564.495349	29409.257246	31.379085
565.011627	29453.339536	31.384103
565.836449	29508.465208	31.389120
566.413544	29540.369345	31.394138
566.832221	29578.572255	31.399156
567.346681	29634.034587	31.404173
568.102995	29681.038737	31.409191
568.757317	29707.894438	31.414208
569.077606	29748.789243	31.419226
569.762049	29782.914501	31.424244
570.136254	29814.704932	31.429261
570.551637	29857.917169	31.434279
571.131742	29895.135404	31.439296
571.427031	29941.933221	31.444314
572.419273	29977.201245	31.449332
572.910696	30020.855663	31.454349
573.321197	30069.020713	31.459367
574.227936	30104.685576	31.464384
574.408354	30166.840644	31.469402
575.373962	30189.597475	31.474420
575.687980	30243.711729	31.479437
576.122127	30278.208833	31.484455
576.478864	30320.500266	31.489472
577.061507	30373.601402	31.494490
577.855625	30413.858237	31.499508
578.314852	30463.267988	31.504525
579.127401	30512.520763	31.509543
579.772524	30557.092982	31.514560
580.201825	30613.717932	31.519578
581.044932	30653.598785	31.524596
581.418634	30697.275340	31.529613
582.110787	30740.737398	31.534631
582.918214	30789.177050	31.539648
583.539410	30828.201669	31.544666
584.446987	30875.013403	31.549684
584.691943	30923.073382	31.554701
585.437486	30952.108812	31.559719
586.117215	30992.282856	31.564736
586.405508	31046.047694	31.569754
586.888063	31076.155928	31.574772
587.471429	31136.849456	31.579789
587.723893	31182.157293	31.584807
588.529245	31232.563877	31.589824
589.319448	31276.404178	31.594842
589.873355	31325.152140	31.599860
590.280309	31373.857456	31.604877
591.034969	31426.042592	31.609895
591.894314	31464.808590	31.614912
592.296574	31518.177005	31.619930
592.893075	31549.164735	31.624948
593.638986	31593.712705	31.629965
594.081072	31659.343219	31.634983
594.640379	31695.019614	31.640000
594.879749	31745.424922	31.645018
595.759052	31803.211662	31.650036
596.087754	31852.387922	31.655053
596.812036	31898.974881	31.660071
597.487948	31938.876046	31.665088
597.912733	32004.901567	31.670106
598.750361	32049.574869	31.675124
599.019434	32088.210959	31.680141
599.524452	32142.193905	31.685159
600.377102	32186.272573	31.690176
601.060391	32235.943579	31.695194
601.755171	32271.902272	31.700212
602.432612	32310.759135	31.705229
602.728169	32349.888102	31.710247
603.686435	32389.021962	31.715264
604.072165	32436.732974	31.720282
604.803708	32484.694829	31.725300
605.131512	32535.271309	31.730317
605.579488	32577.276646	31.735335
606.495371	32612.978642	31.740352
606.722866	32661.725815	31.745370
607.679459	32713.285534	31.750388
608.346963	32756.172118	31.755405
608.930301	32801.067643	31.760423
609.868221	32845.259022	31.765440
610.182492	32894.210577	31.770458
610.594869	32934.805514	31.775476
611.320468	32975.834563	31.780493
611.744489	33035.710927	31.785511
612.133578	33078.373157	31.790528
612.781118	33129.393898	31.795546
613.602714	33172.666843	31.800564
614.156438	33240.320768	31.805581
614.743994	33289.944003	31.810599
615.605178	33328.635310	31.815616
615.912725	33377.953477	31.820634
616.828473	33428.743290	31.825652
617.210300	33483.662886	31.830669
617.227445	33549.644446	31.835687
618.165237	33599.047337	31.840704
618.792970	33653.051949	31.845722
619.743662	33710.003346	31.850740
620.291548	33766.855148	31.855757
620.756990	33825.556620	31.860775
622.092161	33878.415294	31.865792
622.665520	33939.763883	31.870810
622.731468	33973.648015	31.875828
623.519963	34025.331610	31.880845
624.010654	34077.795760	31.885863
624.737907	34139.822033	31.890880
625.683900	34191.654462	31.895898
626.385742	34245.430104	31.900916
627.266910	34290.887562	31.905933
627.396606	34347.573077	31.910951
628.318509	34390.398183	31.915968
628.698646	34434.397327	31.920986
629.234970	34492.829786	31.926004
630.112653	34537.443564	31.931021
630.535281	34582.303317	31.936039
631.512114	34635.476842	31.941056
631.836881	34685.846005	31.946074
632.546480	34735.307546	31.951092
633.612377	34787.718612	31.956109
633.952317	34829.876141	31.961127
634.852986	34876.638904	31.966144
635.090289	34929.075158	31.971162
635.082790	34959.788733	31.976180
636.002877	35012.836935	31.981197
636.528130	35056.091065	31.986215
637.263263	35105.062541	31.991232
637.508552	35160.176529	31.996250
638.156147	35202.703761	32.001268
639.037926	35260.901056	32.006285
639.130684	35319.418084	32.011303
640.406769	35371.015629	32.016320
641.069720	35423.532273	32.021338
641.418483	35484.357977	32.026356
641.895840	35527.595736	32.031373
642.719751	35582.426668	32.036391
643.056001	35638.831465	32.041408
644.129371	35704.675474	32.046426
644.624811	35773.460405	32.051444
645.136831	35824.512601	32.056461
645.578739	35891.939759	32.061479
646.640549	35956.869107	32.066496
647.150322	36016.261753	32.071514
647.647318	36082.708227	32.076532
648.665382	36140.089198	32.081549
649.079620	36194.068282	32.086567
649.956337	36256.362425	32.091584
650.611406	36312.285199	32.096602
651.380292	36364.406427	32.101620
652.188971	36427.642180	32.106637
652.737692	36482.223503	32.111655
653.356246	36525.788202	32.116672
654.130651	36584.347744	32.121690
654.607246	36637.432323	32.126708
655.598228	36713.774207	32.131725
656.110669	36765.491358	32.136743
656.772774	36824.343938	32.141760
657.510268	36877.308911	32.146778
658.045140	36923.366310	32.151796
659.145828	36998.492266	32.156813
659.462746	37039.943284	32.161831
660.127439	37097.364889	32.166848
661.040823	37148.543261	32.171866
661.732702	37200.488591	32.176884
662.665820	37257.486474	32.181901
663.099458	37293.224900	32.186919
663.747462	37340.261838	32.191936
664.147664	37394.658517	32.196954
665.137669	37449.207418	32.201972
665.828649	37492.701614	32.206989
666.006106	37563.277220	32.212007
667.079858	37612.842249	32.217024
667.921610	37665.521936	32.222042
668.048992	37713.481574	32.227060
668.853276	37771.233273	32.232077
669.502508	37828.767053	32.237095
669.886327	37876.005217	32.242112
670.751539	37910.405469	32.247130
671.195542	37972.344464	32.252148
672.058746	38017.187442	32.257165
672.306461	38073.666558	32.262183
672.975947	38130.089749	32.267200
673.523048	38184.807733	32.272218
673.886508	38248.138577	32.277236
674.756449	38292.653269	32.282253
675.586483	38361.934772	32.287271
676.324461	38420.495485	32.292288
676.832257	38475.690526	32.297306
677.315909	38549.001233	32.302324
678.205255	38599.856748	32.307341
678.789652	38675.671554	32.312359
679.182008	38732.183453	32.317376
679.987258	38798.432345	32.322394
680.807627	38878.719947	32.327412
681.713560	38935.264286	32.332429
682.568299	38991.813811	32.337447
682.973783	39058.005956	32.342464
683.539451	39121.599581	32.347482
684.266651	39178.094350	32.352500
685.442906	39253.595197	32.357517
685.955275	39330.241173	32.362535
686.558463	39383.799907	32.367552
687.546271	39428.406054	32.372570
687.950402	39496.675185	32.377588
689.136236	39545.401821	32.382605
689.672557	39619.028870	32.387623
690.691499	39638.665031	32.392640
691.293521	39740.816126	32.397658
691.993478	39777.089804	32.402676
692.999077	39831.746432	32.407693
693.465564	39899.152615	32.412711
694.173209	39948.423284	32.417728
694.627217	40001.495248	32.422746
695.493592	40062.715535	32.427764
695.973802	40121.657467	32.432781
696.897610	40177.146618	32.437799
697.637288	40233.327548	32.442816
698.345347	40286.933937	32.447834
698.677774	40351.841842	32.452852
699.927330	40407.617340	32.457869
700.090490	40466.696094	32.462887
700.554742	40531.373970	32.467904
701.658431	40592.681385	32.472922
701.863730	40653.185900	32.477940
702.668063	40728.441874	32.482957
703.127918	40797.333389	32.487975
703.745309	40845.510878	32.492992
704.653402	40918.742176	32.498010
705.565021	41002.652236	32.503028
706.378297	41029.912556	32.508045
706.628040	41120.381397	32.513063
707.318453	41173.711115	32.518080
708.232436	41225.743843	32.523098
708.514797	41281.576832	32.528116
709.332269	41353.003030	32.533133
710.224771	41421.594798	32.538151
710.501122	41458.215471	32.543168
711.834553	41544.730871	32.548186
712.196159	41613.518313	32.553204
713.073963	41642.833627	32.558221
713.458963	41740.224569	32.563239
714.154462	41780.980348	32.568256
714.903299	41869.012912	32.573274
715.437645	41929.800735	32.578292
715.867604	42026.823433	32.583309
717.150475	42084.114646	32.588327
717.866303	42147.060120	32.593344
718.901572	42219.896683	32.598362
719.417954	42283.297056	32.603380
720.340485	42347.147131	32.608397
721.197953	42417.215133	32.613415
721.939944	42478.738301	32.618432
722.682762	42540.245787	32.623450
723.247075	42602.485289	32.628468
723.987998	42669.339852	32.633485
724.484559	42736.940114	32.638503
725.436835	42795.194741	32.643520
726.421504	42856.112874	32.648538
726.694462	42949.664599	32.653556
728.009528	42985.441869	32.658573
728.768127	43047.730911	32.663591
729.170518	43127.478939	32.668608
730.484827	43179.223619	32.673626
731.058567	43242.015933	32.678644
731.381277	43315.632972	32.683661
731.999467	43381.295435	32.688679
732.660283	43437.806990	32.693696
733.559930	43520.467974	32.698714
734.064336	43565.157169	32.703732
734.903384	43659.584704	32.708749
735.869886	43718.581470	32.713767
736.068312	43794.526179	32.718784
736.829557	43866.432324	32.723802
737.602078	43926.189344	32.728820
738.469596	43997.227427	32.733837
739.484403	44076.696241	32.738855
740.168735	44148.145791	32.743872
741.214893	44199.844748	32.748890
742.001782	44278.524303	32.753908
742.333786	44354.122139	32.758925
743.061145	44413.373850	32.763943
743.832907	44489.123088	32.768960
744.948114	44553.278742	32.773978
745.391637	44624.995717	32.778996
746.001829	44688.102935	32.784013
746.899392	44759.290783	32.789031
747.344838	44820.714935	32.794048
748.261796	44876.083165	32.799066
748.881298	44947.281345	32.804084
749.652441	45006.777330	32.809101
750.587653	45065.313636	32.814119
751.005790	45134.872692	32.819136
751.659852	45185.760022	32.824154
752.590753	45255.777385	32.829172
753.561249	45327.413379	32.834189
754.084032	45398.590948	32.839207
754.800093	45468.908359	32.844224
755.492449	45529.563827	32.849242
756.390833	45595.918822	32.854260
756.638606	45674.772542	32.859277
757.794869	45750.819410	32.864295
758.020697	45816.111889	32.869312
759.161024	45896.610129	32.874330
759.886522	45966.227689	32.879348
760.453686	46047.824235	32.884365
761.768165	46128.150705	32.889383
762.100124	46205.138393	32.894400
762.891823	46273.043036	32.899418
763.320162	46350.621752	32.904436
764.336065	46437.369963	32.909453
765.462786	46504.076964	32.914471
766.303766	46587.288754	32.919488
767.083292	46663.822325	32.924506
767.570973	46742.689999	32.929524
768.408556	46811.359230	32.934541
769.191460	46885.258865	32.939559
769.628210	46966.148506	32.944576
770.659819	47039.037476	32.949594
771.555500	47118.283596	32.954612
772.164301	47205.879697	32.959629
773.477694	47272.023565	32.964647
774.031956	47352.322070	32.969664
774.905563	47414.532747	32.974682
775.795174	47496.860861	32.979700
776.230773	47577.068853	32.984717
777.243089	47647.237446	32.989735
777.685020	47725.252325	32.994752
778.908966	47808.718157	32.999770
779.367832	47888.191878	33.004788
779.957270	47957.132260	33.009805
781.043244	48034.039511	33.014823
781.684596	48117.984467	33.019840
782.693862	48197.772688	33.024858
783.206362	48269.941667	33.029876
783.951062	48337.795527	33.034893
784.853808	48421.274372	33.039911
785.459264	48516.510004	33.044928
786.673686	48584.949498	33.049946
787.364640	48676.351380	33.054964
788.065771	48733.854970	33.059981
788.507024	48825.284744	33.064999
789.467911	48883.571008	33.070016
790.224774	48955.236911	33.075034
790.880633	49029.601208	33.080052
791.798024	49098.364484	33.085069
792.346574	49181.288004	33.090087
792.932706	49245.475670	33.095104
794.123694	49335.977826	33.100122
795.004329	49403.779437	33.105140
795.453908	49475.240766	33.110157
796.467747	49534.716650	33.115175
797.174149	49639.771388	33.120192
798.120426	49707.973923	33.125210
798.845351	49768.957550	33.130228
799.429905	49867.627449	33.135245
800.837941	49935.009519	33.140263
801.300508	50004.079050	33.145280
802.157361	50103.063491	33.150298
802.971687	50156.801776	33.155316
803.612587	50232.987929	33.160333
804.649206	50312.279605	33.165351
805.209943	50397.781800	33.170368
806.360743	50456.920269	33.175386
806.871353	50569.086472	33.180404
807.757566	50613.786529	33.185421
808.622332	50732.896538	33.190439
809.163383	50784.165176	33.195456
810.584691	50877.207224	33.200474
811.273032	50939.503974	33.205492
811.743013	51057.798552	33.210509
812.456381	51125.324096	33.215527
813.756074	51170.969571	33.220544
814.009050	51292.680002	33.225562
814.858703	51359.572531	33.230580
815.866520	51425.950997	33.235597
816.769831	51554.543387	33.240615
817.693023	51604.951998	33.245632
818.109335	51720.788522	33.250650
819.408843	51790.224075	33.255668
820.332240	51863.771838	33.260685
821.149018	51950.342099	33.265703
822.162136	52028.490105	33.270720
822.892221	52112.073724	33.275738
823.720099	52192.947042	33.280756
824.265912	52255.592959	33.285773
825.201516	52343.367539	33.290791
825.630706	52449.596964	33.295808
826.509649	52509.214707	33.300826
827.730646	52605.904872	33.305844
828.338410	52667.166367	33.310861
829.097127	52782.005295	33.315879
829.987857	52848.455007	33.320896
830.841027	52927.446629	33.325914
831.529970	53016.743922	33.330932
831.880682	53104.466965	33.335949
833.099667	53198.124517	33.340967
833.798240	53272.850013	33.345984
834.691771	53362.230077	33.351002
835.469814	53439.837753	33.356020
836.382245	53509.846538	33.361037
836.623917	53602.544457	33.366055
837.711713	53692.251882	33.371072
838.660129	53772.485040	33.376090
839.209622	53858.630434	33.381108
840.215679	53956.952768	33.386125
841.276728	54032.990356	33.391143
841.974184	54133.521606	33.396160
842.811724	54214.134178	33.401178
843.807490	54292.957582	33.406196
844.252317	54387.934411	33.411213
845.279194	54465.254386	33.416231
845.847562	54564.766997	33.421248
846.782751	54650.343454	33.426266
847.962884	54740.218135	33.431284
848.841149	54850.423991	33.436301
850.030193	54904.634506	33.441319
850.593959	55041.979467	33.446336
851.683566	55085.364174	33.451354
852.461514	55198.422543	33.456372
853.198952	55276.697925	33.461389
853.958658	55356.996533	33.466407
855.132523	55465.719741	33.471424
855.909302	55537.430869	33.476442
856.957125	55644.196095	33.481460
857.605271	55697.516541	33.486477
858.781261	55797.526308	33.491495
858.929422	55906.222817	33.496512
860.313750	55976.030297	33.501530
861.094944	56098.437102	33.506548
861.339786	56172.242947	33.511565
862.652682	56258.461307	33.516583
863.626486	56368.342320	33.521600
864.623703	56461.256539	33.526618
865.375861	56543.237736	33.531636
865.819452	56664.262617	33.536653
867.277494	56722.378416	33.541671
867.958678	56853.966851	33.546688
868.382756	56921.339100	33.551706
869.625234	57034.830510	33.556724
870.129415	57119.568527	33.561741
871.292701	57235.315065	33.566759
871.887105	57331.953324	33.571776
873.142485	57412.387270	33.576794
874.245868	57516.588102	33.581812
875.303091	57587.776489	33.586829
876.369051	57702.464979	33.591847
877.557648	57751.588888	33.596864
878.086116	57881.586356	33.601882
879.399832	57932.922750	33.606900
879.820769	58019.916387	33.611917
880.609539	58121.177966	33.616935
881.416928	58177.589848	33.621952
882.230922	58268.398813	33.626970
883.528441	58345.575333	33.631988
884.089764	58411.037023	33.637005
884.985624	58488.208599	33.642023
885.747874	58585.925351	33.647040
886.443390	58650.952973	33.652058
887.438475	58743.067711	33.657076
887.965548	58834.553359	33.662093
888.529270	58913.680095	33.667111
889.575170	59002.826730	33.672128
890.759237	59091.070985	33.677146
891.367864	59205.159647	33.682164
892.435278	59266.063913	33.687181
893.188285	59379.091983	33.692199
893.990563	59500.106796	33.697216
894.287836	59585.236330	33.702234
896.084758	59655.813004	33.707252
896.536995	59777.494655	33.712269
897.525024	59871.178931	33.717287
898.449951	59974.146494	33.722304
899.131627	60077.522730	33.727322
900.408469	60153.614514	33.732340
900.848212	60286.853888	33.737357
901.928050	60358.661855	33.742375
902.967287	60488.915204	33.747392
903.744293	60569.385324	33.752410
904.983440	60677.377446	33.757428
905.475009	60774.059485	33.762445
906.498560	60897.908737	33.767463
907.622178	61005.835890	33.772480
908.543718	61081.369144	33.777498
909.659131	61204.223853	33.782516
910.423413	61297.871958	33.787533
911.177040	61386.085069	33.792551
912.219449	61507.955625	33.797568
913.116172	61606.958244	33.802586
913.971559	61693.356833	33.807604
914.886395	61822.294152	33.812621
915.941361	61915.321259	33.817639
917.056921	62009.687469	33.822656
917.786531	62116.468042	33.827674
919.042232	62206.998580	33.832692
919.794233	62327.363960	33.837709
921.062372	62394.148105	33.842727
921.852094	62527.695052	33.847744
922.387302	62596.611115	33.852762
923.593679	62714.453166	33.857780
924.244776	62800.854611	33.862797
925.461032	62929.663140	33.867815
926.389559	62986.796580	33.872832
927.122107	63128.074374	33.877850
928.366723	63222.593490	33.882868
929.212815	63306.585264	33.887885
930.209746	63411.246495	33.892903
931.421126	63490.785305	33.897920
931.836283	63572.645824	33.902938
932.982790	63683.881476	33.907956
934.051398	63759.563135	33.912973
934.763837	63839.470159	33.917991
935.776552	63927.688681	33.923008
936.697828	64029.854844	33.928026
937.377865	64107.061824	33.933044
937.807145	64208.271425	33.938061
938.853409	64294.430497	33.943079
939.782397	64392.968901	33.948096
940.486472	64513.977931	33.953114
941.514932	64618.511329	33.958132
942.453753	64705.267273	33.963149
943.150073	64808.439763	33.968167
944.251453	64930.840929	33.973184
945.120135	65036.914752	33.978202
946.254478	65131.609354	33.983220
947.179572	65250.323544	33.988237
948.278882	65367.280101	33.993255
949.570512	65463.694615	33.998272
950.231344	65563.942918	34.003290
951.567108	65670.018587	34.008308
952.574105	65763.413306	34.013325
953.426704	65855.080238	34.018343
954.346047	65974.573601	34.023360
955.255568	66058.368461	34.028378
956.569929	66187.085541	34.033396
957.553375	66272.420285	34.038413
958.111598	66372.111175	34.043431
959.363883	66477.086560	34.048448
960.236522	66581.652326	34.053466
960.896094	66699.943992	34.058484
962.104765	66809.962542	34.063501
963.184969	66893.759163	34.068519
964.080653	67007.258635	34.073536
964.907153	67107.125425	34.078554
965.862083	67221.580051	34.083572
967.330268	67324.109512	34.088589
967.633100	67425.804726	34.093607
968.747527	67536.802595	34.098624
969.837308	67648.136666	34.103642
970.834370	67734.603315	34.108660
971.892994	67859.853678	34.113677
973.464301	67963.595647	34.118695
974.036546	68078.564744	34.123712
975.009554	68152.162747	34.128730
976.170257	68275.220136	34.133748
977.718471	68365.284861	34.138765
978.121337	68448.747464	34.143783
979.142376	68560.078767	34.148800
980.285265	68655.882262	34.153818
981.059683	68756.463920	34.158836
982.055511	68858.514418	34.163853
983.352270	68949.550519	34.168871
984.354798	69031.606206	34.173888
984.536991	69122.390833	34.178906
985.569610	69215.643415	34.183924
986.397955	69303.685377	34.188941
986.985771	69398.247831	34.193959
988.250776	69502.299463	34.198976
988.785724	69623.904486	34.203994
989.920214	69719.613476	34.209012
991.133078	69823.719342	34.214029
992.153286	69922.284159	34.219047
992.716873	70028.914099	34.224064
993.710852	70157.367390	34.229082
994.912786	70254.022262	34.234100
996.232801	70364.956201	34.239117
996.790613	70465.555857	34.244135
998.439367	70582.042729	34.249152
999.197216	70682.605360	34.254170
999.954947	70807.423425	34.259188
1000.615258	70913.834298	34.264205
1001.580045	71025.517152	34.269223
1002.612972	71139.508558	34.274240
1003.626023	71254.002922	34.279258
1004.595948	71378.304358	34.284276
1006.103052	71487.995474	34.289293
1006.790374	71612.785621	34.294311
1007.935194	71712.849685	34.299328
1008.717987	71856.568519	34.304346
1009.788486	71955.697883	34.309364
1010.872608	72073.705054	34.314381
1012.028009	72210.878164	34.319399
1012.894432	72297.057235	34.324416
1014.045479	72442.092866	34.329434
1015.138007	72567.791328	34.334452
1016.299746	72663.327088	34.339469
1016.961297	72808.740241	34.344487
1018.725212	72908.560238	34.349504
1019.537657	73011.166996	34.354522
1020.666610	73149.652475	34.359540
1021.861033	73237.723331	34.364557
1022.393911	73373.821896	34.369575
1023.747223	73479.207478	34.374592
1024.531414	73592.576472	34.379610
1025.385113	73717.309176	34.384628
1026.544927	73844.306722	34.389645
1027.545745	73958.509044	34.394663
1028.522492	74075.243477	34.399680
1029.903451	74179.585723	34.404698
1030.824343	74308.134492	34.409716
1032.227167	74411.488688	34.414733
1033.188183	74524.335637	34.419751
1033.958197	74651.254977	34.424768
1035.215821	74753.035264	34.429786
1036.054927	74866.042555	34.434804
1037.035516	74996.816973	34.439821
1037.945932	75088.846547	34.444839
1039.135730	75226.780657	34.449856
1040.137138	75309.380816	34.454874
1041.207386	75422.897953	34.459892
1042.399265	75505.866755	34.464909
1042.965978	75660.618090	34.469927
1044.135801	75719.614849	34.474944
1044.897383	75847.073936	34.479962
1046.048770	75947.613257	34.484980
1047.109198	76064.358604	34.489997
1047.948019	76182.865161	34.495015
1049.165520	76266.009978	34.500032
1050.326781	76426.360410	34.505050
1050.623538	76541.947061	34.510068
1052.155537	76625.896520	34.515085
1052.697778	76781.374484	34.520103
1053.874261	76883.519738	34.525120
1054.840231	77032.966206	34.530138
1055.978062	77161.599823	34.535156
1057.021770	77271.086756	34.540173
1057.923776	77428.572806	34.545191
1058.934347	77531.487169	34.550208
1060.409498	77693.700076	34.555226
1061.252785	77801.262482	34.560244
1062.695220	77947.018401	34.565261
1064.038132	78082.425859	34.570279
1064.951972	78188.721347	34.575296
1065.973987	78316.375756	34.580314
1066.859340	78463.386925	34.585332
1068.168467	78565.456338	34.590349
1069.007425	78721.654075	34.595367
1070.136274	78820.877599	34.600384
1071.385478	78958.833999	34.605402
1072.122391	79101.094992	34.610420
1073.591956	79218.912155	34.615437
1074.635781	79363.654429	34.620455
1076.022739	79483.786996	34.625472
1077.155437	79611.242262	34.630490
1077.744220	79726.655142	34.635508
1079.293237	79866.232347	34.640525
1080.378851	79988.495362	34.645543
1081.544583	80094.988241	34.650560
1082.481452	80237.617203	34.655578
1083.846845	80349.800143	34.660596
1085.216135	80477.716192	34.665613
1086.036512	80620.878339	34.670631
1087.231576	80713.273689	34.675648
1088.240294	80873.101753	34.680666
1089.224190	80968.028694	34.685684
1090.544527	81085.595833	34.690701
1091.108424	81227.703073	34.695719
1092.412638	81349.964677	34.700736
1093.482563	81455.417830	34.705754
1094.610217	81619.796765	34.710772
1095.493436	81712.315709	34.715789
1096.406037	81850.503039	34.720807
1097.845635	81967.228101	34.725824
1098.917455	82067.411921	34.730842
1099.549364	82223.890362	34.735860
1100.840744	82298.412652	34.740877
1101.749532	82430.086853	34.745895
1103.165107	82578.364256	34.750912
1103.958174	82658.093982	34.755930
1105.309213	82793.625940	34.760948
1106.219819	82912.716267	34.765965
1107.330731	83053.231748	34.770983
1108.271745	83159.011163	34.776000
1109.671813	83285.808009	34.781018
1110.297706	83421.844996	34.786036
1111.807396	83565.429869	34.791053
1112.535045	83677.650021	34.796071
1113.916750	83791.574874	34.801088
1115.177076	83952.910173	34.806106
1115.999722	84062.689584	34.811124
1117.389036	84209.623460	34.816141
1117.979095	84338.863083	34.821159
1119.457178	84451.410587	34.826176
1120.800262	84608.527127	34.831194
1121.592873	84736.074208	34.836212
1122.734228	84847.981921	34.841229
1124.144357	85019.714541	34.846247
1124.982917	85133.277815	34.851264
1126.174376	85299.673384	34.856282
1127.023264	85409.348149	34.861300
1128.160360	85574.123302	34.866317
1129.647586	85711.308937	34.871335
1130.702577	85830.007130	34.876352
1131.648126	85988.505931	34.881370
1132.829019	86119.116703	34.886388
1133.890825	86280.665736	34.891405
1135.370412	86400.494611	34.896423
1136.340512	86567.573927	34.901440
1137.562517	86707.634506	34.906458
1138.817723	86840.659575	34.911476
1140.094550	86965.658130	34.916493
1141.392140	87138.924338	34.921511
1142.440034	87249.379976	34.926528
1143.530013	87415.333998	34.931546
1144.855071	87527.884226	34.936564
1146.072520	87693.516623	34.941581
1147.310723	87828.959697	34.946599
1148.539335	87934.464309	34.951616
1149.692913	88090.030588	34.956634
1150.542320	88212.771076	34.961652
1151.698568	88350.728209	34.966669
1152.922504	88499.842701	34.971687
1154.079586	88640.280357	34.976704
1155.415623	88763.559990	34.981722
1156.460460	88897.371126	34.986740
1157.674078	89068.990512	34.991757
1158.604102	89182.756800	34.996775
1159.636387	89292.991450	35.001792
1161.558988	89394.010550	35.006810
1162.252795	89514.721655	35.011828
1163.425929	89646.423867	35.016845
1164.199101	89789.655597	35.021863
1165.645594	89934.849123	35.026880
1166.648123	90064.304401	35.031898
1167.290679	90178.052062	35.036916
1168.488695	90304.265119	35.041933
1169.517996	90433.364196	35.046951
1171.354526	90559.964165	35.051968
1172.424036	90711.610131	35.056986
1173.565418	90878.594450	35.062004
1174.267938	90986.215014	35.067021
1175.811068	91106.306628	35.072039
1176.648965	91293.744332	35.077056
1178.023813	91422.256759	35.082074
1178.836247	91545.705018	35.087092
1180.093214	91726.780746	35.092109
1181.428064	91835.607778	35.097127
1182.111024	92013.728764	35.102144
1183.405237	92144.604634	35.107162
1184.791776	92310.530000	35.112180
1185.685345	92479.235609	35.117197
1187.007940	92604.253108	35.122215
1187.873639	92794.197438	35.127232
1189.521118	92899.229482	35.132250
1190.546634	93111.603972	35.137268
1191.313547	93243.582180	35.142285
1192.882773	93375.768833	35.147303
1193.984622	93599.248679	35.152320
1195.171463	93738.474705	35.157338
1196.838654	93905.271910	35.162356
1198.314682	94043.403921	35.167373
1199.477585	94219.581515	35.172391
1200.722561	94357.967272	35.177408
1202.222851	94522.461669	35.182426
1203.510202	94658.502234	35.187444
1204.493066	94802.169725	35.192461
1206.217126	94981.287618	35.197479
1207.515866	95097.663604	35.202496
1208.680194	95279.858455	35.207514
1209.582233	95394.597521	35.212532
1210.960885	95569.227047	35.217549
1212.524714	95680.301110	35.222567
1213.329444	95846.699647	35.227584
1215.032273	95986.464942	35.232602
1215.917445	96141.669191	35.237620
1216.754848	96277.145921	35.242637
1218.207284	96419.243620	35.247655
1219.499874	96579.136747	35.252672
1220.489602	96718.172308	35.257690
1221.696554	96897.191620	35.262708
1222.808058	97019.294304	35.267725
1224.354441	97166.923280	35.272743
1224.973735	97320.735601	35.277760
1226.509288	97429.172213	35.282778
1227.776757	97612.426005	35.287796
1229.029676	97718.201378	35.292813
1230.263500	97841.181036	35.297831
1231.272205	98010.340274	35.302848
1232.359767	98126.809788	35.307866
1233.299538	98273.688377	35.312884
1234.548164	98450.359972	35.317901
1235.972181	98574.009257	35.322919
1236.678090	98745.702024	35.327936
1238.232018	98882.788560	35.332954
1238.995745	99029.352053	35.337972
1240.327330	99195.432060	35.342989
1241.705600	99376.132856	35.348007
1242.962996	99513.681546	35.353024
1244.378459	99691.873589	35.358042
1245.071863	99837.453824	35.363060
1246.526212	100018.603114	35.368077
1247.889271	100184.122205	35.373095
1248.822397	100335.076884	35.378112
1250.466338	100522.153545	35.383130
1251.930168	100664.921296	35.388148
1252.763189	100854.432561	35.393165
1254.163610	101017.870132	35.398183
1255.082177	101182.922933	35.403200
1256.607407	101357.048445	35.408218
1258.147591	101532.666098	35.413236
1259.154400	101710.635007	35.418253
1260.702925	101883.558605	35.423271
1261.961870	102043.185264	35.428288
1263.413665	102221.100004	35.433306
1264.808339	102390.344010	35.438324
1266.498355	102562.370661	35.443341
1267.980970	102710.988256	35.448359
1269.048229	102872.334178	35.453376
1270.020779	103024.426396	35.458394
1271.273728	103188.339281	35.463412
1272.354694	103370.403035	35.468429
1274.351084	103513.198559	35.473447
1275.291973	103682.403833	35.478464
1276.136250	103838.425938	35.483482
1277.758136	104014.340371	35.488500
1279.184646	104192.508259	35.493517
1280.936388	104355.438799	35.498535
1281.577529	104506.941527	35.503552
1283.050021	104687.263681	35.508570
1284.362369	104824.480705	35.513588
1285.281635	105029.047548	35.518605
1286.713266	105164.956657	35.523623
1288.081953	105348.628954	35.528640
1289.567759	105488.486423	35.533658
1291.291610	105661.739076	35.538676
1292.621513	105829.404431	35.543693
1293.753937	105977.724950	35.548711
1295.089840	106126.444380	35.553728
1296.554001	106253.450517	35.558746
1297.673629	106419.976371	35.563764
1298.728860	106559.130178	35.568781
1300.351966	106675.506734	35.573799
1301.350219	106851.535035	35.578816
1302.562309	106983.825192	35.583834
1303.667375	107127.961340	35.588852
1304.490285	107285.123349	35.593869
1305.777481	107452.762596	35.598887
1307.100139	107602.575534	35.603904
1308.459940	107759.237613	35.608922
1309.742035	107916.729487	35.613940
1310.893366	108095.426017	35.618957
1312.633500	108262.410331	35.623975
1313.476765	108437.088843	35.628992
1314.727482	108605.083680	35.634010
1316.373961	108753.808019	35.639028
1317.516580	108928.480476	35.644045
1318.889274	109106.623986	35.649063
1320.044121	109286.936374	35.654080
1321.493916	109451.633237	35.659098
1322.623550	109634.300368	35.664116
1323.789194	109800.785318	35.669133
1325.299518	109995.736895	35.674151
1326.429174	110160.483108	35.679168
1327.963130	110319.678511	35.684186
1329.147221	110537.497745	35.689204
1330.991268	110728.123360	35.694221
1332.315002	110872.398954	35.699239
1333.362183	111078.053892	35.704256
1335.291639	111250.136695	35.709274
1336.695779	111413.126028	35.714292
1337.715092	111622.081428	35.719309
1339.450046	111771.512724	35.724327
1340.602754	111944.236552	35.729344
1341.731781	112123.156044	35.734362
1343.438678	112294.762467	35.739380
1344.512401	112485.112680	35.744397
1346.412295	112660.172491	35.749415
1347.847354	112837.162144	35.754432
1348.743349	113018.986364	35.759450
1350.119037	113182.004551	35.764468
1351.246698	113364.990896	35.769485
1352.772576	113550.523388	35.774503
1353.951478	113712.848340	35.779520
1355.031772	113915.052555	35.784538
1356.936111	114086.722279	35.789556
1358.558622	114258.399989	35.794573
1359.695715	114451.356996	35.799591
1361.601701	114595.884607	35.804608
1363.082564	114812.067305	35.809626
1364.434409	114962.566253	35.814644
1365.817997	115129.362637	35.819661
1367.195079	115283.759217	35.824679
1368.332489	115449.748525	35.829696
1369.304696	115583.813479	35.834714
1370.758878	115761.339912	35.839732
1371.860839	115900.007461	35.844749
1373.000493	116092.995635	35.849767
1374.073007	116244.122737	35.854784
1375.696747	116430.382681	35.859802
1377.020542	116576.552618	35.864820
1378.108210	116778.436765	35.869837
1379.299158	116936.513406	35.874855
1381.253526	117094.862247	35.879872
1382.289816	117331.321001	35.884890
1383.716850	117485.843351	35.889908
1384.306995	117655.466915	35.894925
1386.693115	117804.818034	35.899943
1387.848674	118045.120244	35.904960
1389.116721	118227.055818	35.909978
1390.741626	118381.526808	35.914996
1391.469191	118607.339796	35.920013
1393.379449	118768.434917	35.925031
1394.581608	118991.478587	35.930048
1395.833652	119155.055097	35.935066
1397.487364	119368.785977	35.940084
1399.133870	119553.228810	35.945101
1400.233206	119738.374095	35.950119
1401.966602	119936.716937	35.955136
1403.259688	120124.284635	35.960154
1405.061072	120310.075942	35.965172
1406.382170	120508.501330	35.970189
1407.669900	120708.592537	35.975207
1409.670392	120888.144554	35.980224
1410.586620	121066.679647	35.985242
1412.409541	121275.111948	35.990260
1413.223639	121482.110476	35.995277
1415.097105	121643.742204	36.000295
1416.401000	121854.781849	36.005312
1417.833194	122038.016173	36.010330
1419.249720	122223.343973	36.015348
1420.765381	122403.388687	36.020365
1422.276878	122625.686034	36.025383
1423.773456	122789.499761	36.030400
1425.079325	123019.368875	36.035418
1427.079272	123179.128132	36.040436
1428.226126	123395.473837	36.045453
1430.238755	123565.201133	36.050471
1431.086140	123738.065754	36.055488
1432.712764	123939.090236	36.060506
1434.396391	124113.230316	36.065524
1435.174287	124305.349028	36.070541
1436.774213	124498.605107	36.075559
1438.129761	124667.671205	36.080576
1439.496396	124881.891478	36.085594
1441.249806	125070.592810	36.090612
1442.697695	125253.416161	36.095629
1443.937300	125452.094229	36.100647
1445.724019	125622.009816	36.105664
1446.894844	125789.313680	36.110682
1448.887432	125945.278009	36.115700
1449.702165	126131.285918	36.120717
1451.453640	126301.464721	36.125735
1452.710280	126450.316132	36.130752
1453.993559	126628.196858	36.135770
1455.451661	126826.748981	36.140788
1457.067514	126985.755931	36.145805
1458.121117	127164.221345	36.150823
1459.718513	127354.344143	36.155840
1460.530935	127543.351576	36.160858
1462.367430	127711.929613	36.165876
1463.763087	127938.355591	36.170893
1465.226066	128108.021491	36.175911
1466.403996	128297.064731	36.180928
1467.465863	128525.081384	36.185946
1469.530847	128700.710547	36.190964
1470.620787	128904.821475	36.195981
1472.350244	129103.245663	36.200999
1473.918020	129319.951885	36.206016
1475.164907	129517.391584	36.211034
1476.633473	129709.160029	36.216052
1478.092075	129919.769450	36.221069
1479.755775	130106.480245	36.226087
1481.145830	130331.178486	36.231104
1482.816525	130534.613728	36.236122
1484.171699	130726.723929	36.241140
1485.541148	130952.367948	36.246157
1487.463226	131165.320261	36.251175
1488.960784	131366.673335	36.256192
1490.153854	131574.030779	36.261210
1492.005057	131784.819947	36.266228
1493.241389	131999.167138	36.271245
1494.755417	132199.839416	36.276263
1496.436374	132405.364411	36.281280
1498.004268	132624.237416	36.286298
1499.624994	132833.107230	36.291316
1501.204893	133035.713462	36.296333
1502.643146	133250.975641	36.301351
1504.330196	133467.264215	36.306368
1505.842922	133675.701262	36.311386
1507.402271	133874.870447	36.316404
1508.793886	134082.835569	36.321421
1509.935290	134295.669402	36.326439
1511.830029	134515.936801	36.331456
1513.258486	134726.409519	36.336474
1514.737801	134919.960247	36.341492
1516.551125	135145.959923	36.346509
1518.254726	135348.626260	36.351527
1519.579996	135558.779342	36.356544
1520.950975	135769.724973	36.361562
1522.776325	135964.634240	36.366580
1524.372078	136180.869068	36.371597
1525.630528	136378.342075	36.376615
1527.327728	136571.070954	36.381632
1528.585852	136772.804306	36.386650
1529.710401	136945.782980	36.391668
1531.455391	137133.743459	36.396685
1533.061585	137334.335635	36.401703
1534.376329	137530.324901	36.406720
1535.359265	137733.261737	36.411738
1536.901692	137913.415451	36.416756
1538.463906	138155.964751	36.421773
1539.911745	138334.463345	36.426791
1541.478462	138565.914433	36.431808
1542.948728	138772.468670	36.436826
1544.399228	138989.165497	36.441844
1546.017886	139191.593194	36.446861
1547.425004	139423.253755	36.451879
1549.174703	139636.080628	36.456896
1550.440594	139862.355762	36.461914
1552.054572	140078.198154	36.466932
1553.786685	140304.757431	36.471949
1555.103581	140526.353132	36.476967
1556.843307	140769.339142	36.481984
1558.750479	140978.716113	36.487002
1560.613204	141202.790128	36.492020
1561.805320	141435.653708	36.497037
1563.379142	141655.544015	36.502055
1565.618724	141869.132721	36.507072
1566.813201	142102.837533	36.512090
1568.081073	142346.240716	36.517108
1569.859205	142559.844216	36.522125
1571.448334	142781.501948	36.527143
1572.876714	142996.913096	36.532160
1574.583980	143245.462771	36.537178
1576.341267	143473.435971	36.542196
1577.864600	143675.883591	36.547213
1579.102306	143924.880920	36.552231
1581.217439	144143.955410	36.557248
1582.560644	144380.721289	36.562266
1584.092176	144600.005788	36.567284
1586.158969	144840.374002	36.572301
1587.550261	145069.469172	36.577319
1589.107233	145293.710491	36.582336
1590.912130	145525.519194	36.587354
1592.476837	145778.408828	36.592372
1593.921660	145982.316332	36.597389
1595.532032	146239.245908	36.602407
1597.437549	146432.841361	36.607424
1598.321816	146692.475799	36.612442
1600.457521	146897.014725	36.617460
1601.945668	147166.266824	36.622477
1603.632024	147370.867520	36.627495
1605.276925	147632.112832	36.632512
1607.147959	147831.680130	36.637530
1608.672559	148084.277782	36.642548
1610.532660	148282.505971	36.647565
1611.984643	148541.013288	36.652583
1613.590330	148720.460090	36.657600
1615.018111	148959.883814	36.662618
1616.580432	149144.942954	36.667636
1617.973845	149383.779502	36.672653
1619.631272	149579.221011	36.677671
1620.989127	149805.630348	36.682688
1622.452199	150005.364768	36.687706
1624.322452	150213.960446	36.692724
1625.725585	150453.716142	36.697741
1627.428725	150655.723712	36.702759
1629.173765	150910.882105	36.707776
1630.198857	151121.278586	36.712794
1631.851810	151356.627556	36.717812
1633.806273	151574.308421	36.722829
1635.062123	151835.814503	36.727847
1636.345097	152058.105826	36.732864
1638.556839	152273.126177	36.737882
1639.706315	152549.500678	36.742900
1641.592178	152764.626709	36.747917
1643.372386	153038.154000	36.752935
1645.119850	153251.542915	36.757952
1646.981914	153525.188018	36.762970
1648.309602	153754.989285	36.767988
1650.330387	154005.956716	36.773005
1651.798897	154228.397997	36.778023
1653.839777	154497.394993	36.783040
1655.793174	154721.575624	36.788058
1657.163686	154966.669124	36.793076
1659.034559	155210.505807	36.798093
1660.776184	155450.459613	36.803111
1662.202687	155693.939272	36.808128
1664.028195	155941.490777	36.813146
1665.512977	156184.825243	36.818164
1667.378875	156423.992784	36.823181
1668.919164	156669.528139	36.828199
1670.522952	156919.391628	36.833216
1672.004439	157160.400535	36.838234
1673.820749	157406.607431	36.843252
1675.713951	157664.165112	36.848269
1677.245593	157927.931956	36.853287
1679.207419	158156.673395	36.858304
1681.037928	158401.388909	36.863322
1682.695401	158658.890018	36.868340
1684.913683	158895.685667	36.873357
1686.211861	159131.766759	36.878375
1687.836948	159370.194172	36.883392
1689.758462	159613.737175	36.888410
1691.393764	159894.469239	36.893428
1693.375929	160098.949285	36.898445
1694.684440	160377.847666	36.903463
1696.464538	160583.884334	36.908480
1697.947551	160852.246215	36.913498
1699.587955	161073.918367	36.918516
1701.101881	161347.630559	36.923533
1702.966827	161574.811914	36.928551
1704.827052	161802.984625	36.933568
1706.172088	162031.088422	36.938586
1708.198524	162248.914843	36.943604
1709.554169	162461.624248	36.948621
1711.254844	162723.168313	36.953639
1713.127724	162922.431749	36.958656
1714.668974	163182.939200	36.963674
1716.234204	163394.733120	36.968692
1717.968582	163644.458903	36.973709
1719.329058	163887.879322	36.978727
1721.053092	164121.693912	36.983744
1722.303930	164378.603587	36.988762
1724.275536	164628.399932	36.993780
1726.119853	164864.419619	36.998797
1727.644422	165152.946852	37.003815
1729.593016	165385.605132	37.008832
1731.210472	165645.192269	37.013850
1732.732941	165920.865519	37.018868
1734.339099	166161.636695	37.023885
1736.211395	166438.057286	37.028903
1738.108238	166692.851274	37.033920
1739.765680	166969.627009	37.038938
1741.459633	167217.810784	37.043956
1743.166010	167499.973092	37.048973
1745.295272	167780.218593	37.053991
1747.042154	168036.478784	37.059008
1749.002471	168298.414492	37.064026
1750.564004	168589.131399	37.069044
1752.469831	168831.901580	37.074061
1754.151871	169131.317328	37.079079
1755.964645	169389.136341	37.084096
1757.689188	169649.063986	37.089114
1759.575659	169944.927474	37.094132
1761.404361	170179.981099	37.099149
1762.893708	170484.093167	37.104167
1765.016055	170709.539366	37.109184
1767.071705	171014.986377	37.114202
1768.098022	171285.640230	37.119220
1770.405821	171556.828247	37.124237
1771.944887	171860.296295	37.129255
1773.961401	172091.729207	37.134272
1775.861861	172393.494980	37.139290
1777.702523	172652.409537	37.144308
1779.713732	172924.313739	37.149325
1781.360595	173190.074548	37.154343
1782.681049	173485.953301	37.159360
1784.992535	173727.763699	37.164378
1786.287637	174030.449935	37.169396
1788.166276	174273.677029	37.174413
1789.913112	174585.619701	37.179431
1791.804860	174836.396143	37.184448
1793.376497	175139.389372	37.189466
1795.853384	175371.237695	37.194484
1797.776667	175679.329663	37.199501
1798.778709	175955.524952	37.204519
1800.891290	176187.410403	37.209536
1803.035024	176465.927112	37.214554
1804.434727	176706.707608	37.219572
1806.111158	176967.325291	37.224589
1807.750835	177195.472896	37.229607
1809.206562	177496.789360	37.234624
1810.578297	177741.551266	37.239642
1812.642687	177997.077248	37.244660
1814.184163	178303.968158	37.249677
1816.422701	178566.536593	37.254695
1817.706065	178847.806755	37.259712
1820.046746	179142.054848	37.264730
1821.714937	179437.236416	37.269748
1823.632042	179699.431599	37.274765
1825.254582	179972.548252	37.279783
1826.983512	180279.550706	37.284800
1828.690053	180548.458176	37.289818
1830.441312	180862.705884	37.294836
1833.039645	181122.276872	37.299853
1834.488429	181425.906343	37.304871
1836.338779	181685.815153	37.309888
1838.295305	182020.339379	37.314906
1839.755694	182307.110864	37.319924
1841.766439	182571.998637	37.324941
1843.788524	182901.761186	37.329959
1845.680531	183163.385140	37.334976
1847.840539	183483.702757	37.339994
1849.443752	183808.361730	37.345012
1851.445677	184068.844345	37.350029
1853.324022	184356.324202	37.355047
1855.036609	184671.950503	37.360064
1857.768316	184963.854109	37.365082
1859.131714	185275.555801	37.370100
1860.582062	185557.439371	37.375117
1862.921604	185834.184080	37.380135
1864.458266	186177.358829	37.385152
1866.297374	186458.742199	37.390170
1868.537101	186751.433376	37.395188
1870.070929	187079.134385	37.400205
1872.727714	187352.716392	37.405223
1874.211363	187661.458717	37.410240
1876.271961	187998.967875	37.415258
1877.764557	188274.960816	37.420276
1880.149811	188576.168026	37.425293
1881.707872	188882.305254	37.430311
1883.824714	189168.978168	37.435328
1885.780538	189485.893478	37.440346
1887.962395	189751.849415	37.445364
1889.522206	190082.841523	37.450381
1891.409237	190357.464332	37.455399
1893.752766	190666.369192	37.460416
1895.271285	190974.899359	37.465434
1897.624977	191232.473283	37.470452
1899.539610	191558.076587	37.475469
1901.451900	191868.009420	37.480487
1902.975316	192119.552156	37.485504
1905.028351	192366.113479	37.490522
1906.922859	192676.396946	37.495540
1908.660256	192927.668770	37.500557
1910.674976	193177.108434	37.505575
1911.986135	193495.586553	37.510592
1914.058757	193756.835418	37.515610
1916.084845	194005.351008	37.520628
1917.891873	194309.211473	37.525645
1919.665831	194626.544643	37.530663
1921.437343	194892.301942	37.535680
1923.684187	195138.478289	37.540698
1925.187633	195484.123912	37.545716
1927.086146	195769.563120	37.550733
1928.935365	196052.029185	37.555751
1930.324520	196353.366465	37.560768
1932.799659	196656.119684	37.565786
1934.173479	196974.546397	37.570804
1936.472664	197253.685836	37.575821
1938.355156	197610.302395	37.580839
1940.267184	197886.777862	37.585856
1942.343263	198187.052224	37.590874
1944.075655	198539.954723	37.595892
1946.063049	198823.619765	37.600909
1948.548836	199182.232858	37.605927
1949.708210	199479.550370	37.610944
1952.086770	199793.696988	37.615962
1953.860072	200127.120269	37.620980
1956.152095	200446.907348	37.625997
1957.664584	200773.293406	37.631015
1959.964664	201074.145076	37.636032
1962.252131	201421.533213	37.641050
1963.772610	201770.136869	37.646068
1966.223903	202065.918132	37.651085
1968.341048	202387.991048	37.656103
1969.951512	202755.220417	37.661120
1971.942457	203060.282739	37.666138
1974.283861	203358.017734	37.671156
1976.195533	203686.287112	37.676173
1978.161241	204037.208028	37.681191
1980.242911	204392.834795	37.686208
1982.345010	204720.051756	37.691226
1984.395449	205017.384665	37.696244
1986.486301	205336.254350	37.701261
1988.256912	205651.546115	37.706279
1990.523388	205983.060146	37.711296
1992.689021	206330.599422	37.716314
1994.745155	206616.464099	37.721332
1996.581464	206967.372594	37.726349
1998.582916	207275.857726	37.731367
2000.424019	207617.730918	37.736384
2002.582138	207920.951732	37.741402
2004.772060	208249.443955	37.746420
2006.703620	208573.840503	37.751437
2008.923748	208882.184966	37.756455
2010.628221	209180.634705	37.761472
2013.055332	209479.669473	37.766490
2014.930593	209754.584072	37.771508
2016.841993	210058.768745	37.776525
2018.918577	210362.801758	37.781543
2020.661177	210631.698472	37.786560
2022.373535	210960.763416	37.791578
2024.519771	211252.107264	37.796596
2026.277413	211557.440814	37.801613
2028.590393	211872.475836	37.806631
2029.725368	212183.763729	37.811648
2031.626016	212506.471838	37.816666
2033.842810	212838.614967	37.821684
2035.384909	213154.057886	37.826701
2037.411735	213492.912387	37.831719
2039.248899	213827.380627	37.836736
2041.686995	214154.823347	37.841754
2043.483342	214520.126936	37.846772
2045.162626	214843.821210	37.851789
2047.563413	215211.800420	37.856807
2049.757692	215549.889831	37.861824
2051.294127	215902.863559	37.866842
2053.866102	216266.784005	37.871860
2056.083899	216607.998216	37.876877
2058.311554	216958.607823	37.881895
2059.717868	217312.269663	37.886912
2062.180632	217677.027453	37.891930
2064.584277	218034.978505	37.896948
2066.450414	218383.456130	37.901965
2068.949820	218729.003670	37.906983
2071.080944	219092.437454	37.912000
2073.431872	219446.518799	37.917018
2075.540982	219797.377161	37.922036
2077.797929	220152.708461	37.927053
2079.711891	220494.395904	37.932071
2082.249189	220845.191380	37.937088
2084.365194	221193.934940	37.942106
2086.410476	221532.254326	37.947124
2088.466494	221881.124884	37.952141
2091.282657	222229.825697	37.957159
2093.211355	222566.949287	37.962176
2095.049076	222911.872265	37.967194
2097.493982	223250.643824	37.972212
2099.722170	223594.784172	37.977229
2101.843043	223922.931508	37.982247
2103.737060	224309.753546	37.987264
2105.709587	224666.065325	37.992282
2107.999420	225009.795764	37.997300
2109.655896	225351.418731	38.002317
2111.920827	225686.927889	38.007335
2114.105910	226035.783831	38.012352
2116.148555	226381.997297	38.017370
2118.509490	226717.914496	38.022388
2120.332274	227074.870109	38.027405
2122.586196	227400.597851	38.032423
2124.304507	227731.033915	38.037440
2126.545912	228055.293196	38.042458
2128.820692	228365.783577	38.047476
2130.419726	228700.254950	38.052493
2132.844658	229019.333288	38.057511
2134.643724	229337.851747	38.062528
2136.531957	229666.388945	38.067546
2138.494053	230002.610904	38.072564
2140.577947	230352.351399	38.077581
2142.793011	230674.643639	38.082599
2144.571225	231031.216274	38.087616
2146.948452	231375.682409	38.092634
2149.095913	231715.894131	38.097652
2150.759322	232088.387830	38.102669
2153.311331	232429.147555	38.107687
2155.454850	232794.812187	38.112704
2157.347343	233147.920771	38.117722
2159.723143	233508.014611	38.122740
2161.867173	233877.442197	38.127757
2164.091722	234232.051378	38.132775
2166.221005	234613.979922	38.137792
2168.087351	234982.058822	38.142810
2170.891680	235339.678624	38.147828
2172.632908	235713.088302	38.152845
2174.753284	236097.538367	38.157863
2176.803617	236472.324124	38.162880
2179.128047	236844.197725	38.167898
2181.632363	237224.501914	38.172916
2183.747531	237612.107861	38.177933
2186.127306	237981.309824	38.182951
2188.607996	238363.374362	38.187968
2190.666836	238755.539795	38.192986
2193.155201	239119.267600	38.198004
2194.940730	239503.935473	38.203021
2197.482695	239877.537584	38.208039
2200.188024	240249.768855	38.213056
2201.932553	240641.279554	38.218074
2204.365982	241006.368322	38.223092
2206.302148	241383.601946	38.228109
2209.172803	241758.580412	38.233127
2211.241813	242142.119931	38.238144
2213.331610	242519.764585	38.243162
2215.785848	242875.483198	38.248180
2218.055859	243271.161008	38.253197
2220.344172	243640.420982	38.258215
2222.399879	244021.987241	38.263232
2224.828755	244401.463444	38.268250
2226.976050	244758.404453	38.273268
2229.324840	245155.929842	38.278285
2231.588016	245511.889304	38.283303
2233.977663	245886.905519	38.288320
2236.024770	246271.273733	38.293338
2238.322357	246639.473830	38.298356
2240.248493	247005.346119	38.303373
2242.538073	247378.324782	38.308391
2245.108829	247729.161013	38.313408
2246.961748	248077.139995	38.318426
2249.170647	248414.267909	38.323444
2251.092127	248765.031764	38.328461
2253.692207	249110.354598	38.333479
2255.757068	249460.868727	38.338496
2257.882127	249828.672395	38.343514
2260.057383	250174.700006	38.348532
2261.868963	250543.291687	38.353549
2264.374156	250904.966651	38.358567
2266.827394	251265.659996	38.363584
2268.939487	251635.959212	38.368602
2270.718446	251999.961651	38.373620
2273.044078	252376.553643	38.378637
2275.243162	252764.190878	38.383655
2277.598913	253145.148856	38.388672
2279.424719	253535.615754	38.393690
2281.965582	253917.358876	38.398708
2284.246866	254315.350393	38.403725
2286.918291	254704.517203	38.408743
2289.267998	255092.491106	38.413760
2291.180086	255489.654518	38.418778
2293.669589	255882.891453	38.423796
2296.188760	256281.128684	38.428813
2298.426572	256671.841410	38.433831
2300.934678	257066.423964	38.438848
2303.279768	257479.271976	38.443866
2305.931280	257867.457253	38.448884
2307.863417	258261.472791	38.453901
2310.480869	258654.034030	38.458919
2312.832047	259048.594129	38.463936
2314.974411	259457.210197	38.468954
2317.540851	259851.229418	38.473972
2319.500254	260267.826833	38.478989
2321.931920	260662.300510	38.484007
2324.353083	261062.161816	38.489024
2326.662052	261471.211891	38.494042
2329.450782	261866.164160	38.499060
2331.637232	262275.793672	38.504077
2333.954198	262686.038129	38.509095
2336.819399	263080.751263	38.514112
2338.784579	263491.586005	38.519130
2341.373725	263892.516809	38.524148
2343.447172	264291.599206	38.529165
2346.070114	264697.606193	38.534183
2348.563661	265087.706431	38.539200
2350.532210	265506.214728	38.544218
2353.222392	265904.134183	38.549236
2355.254913	266308.788491	38.554253
2357.419657	266720.230273	38.559271
2360.210269	267122.148656	38.564288
2362.303585	267527.810573	38.569306
2365.093611	267934.530947	38.574324
2367.277460	268334.768289	38.579341
2369.561721	268736.996872	38.584359
2372.032488	269113.081615	38.589376
2373.849607	269487.796809	38.594394
2376.247691	269863.106032	38.599412
2378.813590	270242.478801	38.604429
2380.948749	270629.541044	38.609447
2383.298112	271007.144893	38.614464
2385.416240	271398.300149	38.619482
2387.693505	271782.342815	38.624500
2389.902854	272190.123149	38.629517
2392.190779	272585.595945	38.634535
2394.663072	272972.554917	38.639552
2397.081003	273388.304666	38.644570
2399.257395	273793.880637	38.649588
2401.450180	274202.756541	38.654605
2404.102335	274620.095259	38.659623
2406.360360	275035.083175	38.664640
2408.918365	275454.850237	38.669658
2411.474965	275871.213487	38.674676
2413.846713	276290.070168	38.679693
2416.169220	276719.959723	38.684711
2419.032081	277141.151849	38.689728
2421.157745	277569.294275	38.694746
2423.553657	277989.899795	38.699764
2426.111461	278423.638532	38.704781
2427.820130	278865.361372	38.709799
2430.788534	279288.695612	38.714816
2433.283536	279735.450430	38.719834
2435.875301	280176.092923	38.724852
2438.352696	280608.497251	38.729869
2441.062196	281057.529174	38.734887
2443.851374	281478.299725	38.739904
2446.287326	281936.926134	38.744922
2448.664779	282350.699298	38.749940
2451.115890	282786.510562	38.754957
2453.841599	283218.289683	38.759975
2456.311465	283657.679179	38.764992
2458.767656	284098.518462	38.770010
2461.374991	284522.033836	38.775028
2464.126481	284958.176767	38.780045
2466.523137	285384.595299	38.785063
2469.569174	285817.845560	38.790080
2471.747510	286255.602196	38.795098
2474.141551	286688.091138	38.800116
2476.952291	287117.312779	38.805133
2479.038031	287553.863249	38.810151
2481.678411	287974.804080	38.815168
2484.130424	288403.420521	38.820186
2486.594597	288835.540076	38.825204
2488.969283	289265.971230	38.830221
2491.328435	289701.281584	38.835239
2494.266728	290132.028645	38.840256
2496.792371	290568.733884	38.845274
2498.951635	291003.692902	38.850292
2501.929465	291424.143612	38.855309
2504.106898	291854.195654	38.860327
2506.357279	292251.212055	38.865344
2509.093682	292661.207728	38.870362
2511.593996	293040.604701	38.875380
2514.209717	293440.050734	38.880397
2516.743143	293848.120544	38.885415
2519.045760	294238.165106	38.890432
2520.978127	294637.844328	38.895450
2523.613161	295042.060107	38.900468
2526.066281	295450.952552	38.905485
2528.407604	295863.189599	38.910503
2531.060221	296283.479776	38.915520
2533.216160	296710.071274	38.920538
2535.589303	297129.895899	38.925556
2538.340185	297548.313460	38.930573
2540.784006	298000.487070	38.935591
2543.311428	298421.630684	38.940608
2545.968353	298867.748159	38.945626
2548.378621	299314.157612	38.950644
2550.928482	299757.139988	38.955661
2553.128040	300203.148703	38.960679
2555.590591	300648.022307	38.965696
2558.151843	301104.589144	38.970714
2561.046796	301552.871785	38.975732
2563.479287	302014.181096	38.980749
2565.874327	302493.580652	38.985767
2568.599684	302946.102777	38.990784
2571.139563	303419.862824	38.995802
2573.929331	303882.430741	39.000820
2576.952996	304343.690096	39.005837
2579.141726	304812.471879	39.010855
2581.662793	305286.965428	39.015872
2584.331975	305757.674600	39.020890
2587.012174	306228.024802	39.025908
2590.076550	306708.701297	39.030925
2592.173561	307176.244896	39.035943
2594.934470	307644.545265	39.040960
2597.359644	308126.130615	39.045978
2599.998806	308608.493043	39.050996
2603.126202	309084.172271	39.056013
2606.035038	309569.307647	39.061031
2608.548909	310035.580801	39.066048
2611.195535	310503.888486	39.071066
2614.000220	310977.147599	39.076084
2616.740246	311448.484672	39.081101
2619.062829	311914.958454	39.086119
2621.768420	312384.900152	39.091136
2624.703032	312868.544555	39.096154
2627.361139	313345.626885	39.101172
2630.256560	313804.483890	39.106189
2632.766596	314276.099408	39.111207
2635.164415	314734.066095	39.116224
2637.750797	315215.799428	39.121242
2640.469509	315684.632530	39.126260
2643.248956	316157.796996	39.131277
2645.634100	316617.789214	39.136295
2648.280464	317055.870140	39.141312
2651.113606	317488.585961	39.146330
2653.415766	317948.280382	39.151348
2656.251539	318377.817109	39.156365
2658.675474	318813.817366	39.161383
2661.267804	319251.058835	39.166400
2663.454306	319693.746813	39.171418
2666.067135	320131.971429	39.176436
2668.618029	320597.226411	39.181453
2670.750338	321067.218382	39.186471
2673.463087	321531.223891	39.191488
2676.151449	322005.389583	39.196506
2678.858333	322479.092664	39.201524
2681.531434	322943.427215	39.206541
2683.665102	323437.355331	39.211559
2686.489126	323919.539792	39.216576
2689.247844	324411.356987	39.221594
2691.881870	324922.745940	39.226612
2694.908710	325397.448803	39.231629
2697.150752	325908.893754	39.236647
2699.938765	326401.100838	39.241664
2703.206570	326906.231356	39.246682
2705.790375	327417.891987	39.251700
2708.497703	327913.835640	39.256717
2711.433035	328422.132738	39.261735
2714.476346	328923.908376	39.266752
2716.947433	329433.491295	39.271770
2719.635450	329928.434709	39.276788
2722.848382	330442.464360	39.281805
2725.003493	330949.471494	39.286823
2727.941961	331465.518283	39.291840
2730.821859	331966.588473	39.296858
2733.699661	332481.571169	39.301876
2736.740079	332997.971856	39.306893
2739.422449	333515.288878	39.311911
2742.090334	334017.114736	39.316928
2744.852121	334545.025871	39.321946
2747.899317	335048.460185	39.326964
2750.829221	335560.822118	39.331981
2753.580752	336074.554243	39.336999
2756.460537	336583.615439	39.342016
2759.821982	337088.076778	39.347034
2762.630880	337584.648836	39.352052
2765.518590	338095.169956	39.357069
2768.292266	338577.114668	39.362087
2771.061816	339079.800926	39.367104
2773.783486	339583.176405	39.372122
2776.477013	340089.243792	39.377140
2779.693682	340579.888511	39.382157
2782.592254	341077.079676	39.387175
2785.461973	341568.660268	39.392192
2788.122797	342057.096321	39.397210
2790.984750	342549.381271	39.402228
2793.638890	343034.992364	39.407245
2796.366371	343529.093347	39.412263
2799.162255	343985.984571	39.417280
2801.852333	344434.942364	39.422298
2804.437059	344904.681343	39.427316
2807.347728	345354.409689	39.432333
2809.767712	345822.974176	39.437351
2812.588811	346277.177942	39.442368
2815.308854	346741.270009	39.447386
2817.442330	347217.332603	39.452404
2819.906071	347690.013200	39.457421
2822.580805	348187.332799	39.462439
2825.471721	348678.292440	39.467456
2828.160250	349168.670540	39.472474
2830.321755	349679.614662	39.477492
2833.454075	350181.921358	39.482509
2836.214357	350701.570242	39.487527
2838.820591	351226.239559	39.492544
2841.654490	351742.211286	39.497562
2844.459168	352275.013133	39.502580
2847.480488	352802.698362	39.507597
2850.200189	353324.232204	39.512615
2852.890792	353864.905419	39.517632
2855.877395	354394.179425	39.522650
2858.868206	354959.137267	39.527668
2861.888865	355485.247113	39.532685
2864.925726	356040.768418	39.537703
2867.745042	356589.794620	39.542720
2870.936078	357127.333710	39.547738
2873.430425	357686.197203	39.552756
2876.914104	358230.150686	39.557773
2879.731761	358768.974917	39.562791
2882.625750	359335.015813	39.567808
2885.869043	359877.263174	39.572826
2888.805970	360431.076039	39.577844
2891.923117	360969.320901	39.582861
2894.814797	361515.514161	39.587879
2897.975459	362067.597578	39.592896
2900.970606	362606.300092	39.597914
2903.784311	363155.735405	39.602932
2906.769996	363689.579434	39.607949
2910.053867	364236.465771	39.612967
2912.589580	364790.290956	39.617984
2915.784112	365322.458790	39.623002
2918.885619	365886.713235	39.628020
2921.521154	366421.748276	39.633037
2924.543748	366968.617805	39.638055
2927.472133	367511.765097	39.643072
2930.356213	368051.994414	39.648090
2932.958629	368606.904063	39.653108
2936.323637	369157.854178	39.658125
2939.256496	369705.313096	39.663143
2941.934707	370260.951026	39.668160
2945.442983	370798.814527	39.673178
2948.514660	371352.422193	39.678196
2951.297494	371901.475562	39.683213
2954.367669	372425.634783	39.688231
2956.944325	372953.341855	39.693248
2960.037348	373459.392835	39.698266
2962.604977	373963.998422	39.703284
2965.763960	374468.072946	39.708301
2968.536720	374969.715902	39.713319
2971.355006	375492.709239	39.718336
2974.349709	375999.150637	39.723354
2976.957614	376523.407296	39.728372
2979.700863	377038.197511	39.733389
2982.758089	377570.539120	39.738407
2985.109707	378108.643034	39.743424
2988.414642	378641.260997	39.748442
2991.647504	379181.062985	39.753460
2994.352827	379731.266609	39.758477
2997.072253	380285.265712	39.763495
2999.776538	380841.618676	39.768512
3003.032832	381397.774835	39.773530
3005.783755	381978.940109	39.778548
3008.756877	382530.659868	39.783565
3012.006980	383103.459096	39.788583
3014.700292	383680.092150	39.793600
3017.772011	384255.134509	39.798618
3020.665875	384859.697443	39.803636
3023.782888	385424.644190	39.808653
3026.723024	386018.248217	39.813671
3029.786666	386617.910838	39.818688
3032.892679	387222.452392	39.823706
3036.005200	387818.511195	39.828724
3039.513406	388417.642760	39.833741
3042.718384	389021.834373	39.838759
3045.249844	389629.723982	39.843776
3048.810934	390214.968950	39.848794
3051.773100	390826.295453	39.853812
3055.001099	391439.370034	39.858829
3058.426641	392025.392742	39.863847
3061.162055	392635.785344	39.868864
3064.391555	393235.057231	39.873882
3067.404696	393843.736245	39.878900
3070.545412	394446.729124	39.883917
3073.940261	395052.333920	39.888935
3077.001770	395660.212286	39.893952
3080.397620	396278.373075	39.898970
3083.386743	396871.381182	39.903988
3086.391538	397477.131136	39.909005
3089.743592	398077.388792	39.914023
3092.547244	398696.511554	39.919040
3095.745694	399299.585988	39.924058
3098.890430	399903.266417	39.929076
3102.056724	400522.703191	39.934093
3105.479661	401121.601076	39.939111
3108.393461	401726.197084	39.944128
3111.393240	402341.137830	39.949146
3114.811411	402945.149463	39.954164
3117.718723	403547.379766	39.959181
3120.524968	404139.752653	39.964199
3123.412424	404735.270594	39.969216
3126.973193	405280.576612	39.974234
3129.892933	405851.883159	39.979252
3132.691938	406424.922197	39.984269
3135.965892	406986.746939	39.989287
3138.692851	407571.918838	39.994304
3141.751710	408132.387928	39.999322
3144.838344	408731.828420	40.004340
3147.680941	409327.823095	40.009357
3150.972081	409920.693453	40.014375
3153.590720	410528.081045	40.019392
3157.009539	411097.791663	40.024410
3160.164431	411733.711669	40.029428
3163.244572	412331.789205	40.034445
3166.851164	412936.183732	40.039463
3169.268723	413580.823556	40.044480
3172.747273	414179.307683	40.049498
3175.984369	414801.133707	40.054516
3178.907086	415462.632375	40.059533
3182.160286	416066.587556	40.064551
3185.270867	416736.770564	40.069568
3188.723133	417347.535084	40.074586
3191.603571	418003.280550	40.079604
3194.605367	418661.044313	40.084621
3198.138235	419299.476272	40.089639
3200.935221	419948.323127	40.094656
3204.192458	420600.426899	40.099674
3207.643217	421286.487999	40.104692
3210.818983	421944.299647	40.109709
3214.274468	422618.469477	40.114727
3217.333283	423276.724073	40.119744
3220.714952	423954.419961	40.124762
3223.722787	424635.553050	40.129780
3227.206017	425299.645566	40.134797
3230.576655	425964.347652	40.139815
3233.458105	426662.195219	40.144832
3236.922654	427332.421928	40.149850
3240.260527	428015.165604	40.154868
3243.464622	428695.430551	40.159885
3246.845992	429371.571894	40.164903
3250.173765	430078.834261	40.169920
3253.989356	430748.513954	40.174938
3257.059981	431430.629117	40.179956
3260.130722	432139.066929	40.184973
3263.762341	432799.731812	40.189991
3266.752258	433485.832703	40.195008
3269.809499	434193.760469	40.200026
3273.593567	434869.442025	40.205044
3276.521699	435557.219302	40.210061
3279.907448	436258.301633	40.215079
3283.034037	436937.678687	40.220096
3286.547808	437634.752193	40.225114
3290.118023	438313.667374	40.230132
3293.067320	439003.296909	40.235149
3296.211406	439708.828008	40.240167
3299.332593	440331.093234	40.245184
3302.456703	441010.612797	40.250202
3305.985847	441648.832096	40.255220
3308.949269	442292.542062	40.260237
3312.000758	442951.816049	40.265255
3315.143390	443629.538230	40.270272
3318.641803	444263.997602	40.275290
3321.913268	444969.812119	40.280308
3324.828115	445610.454260	40.285325
3328.129098	446318.300036	40.290343
3331.218269	446969.610741	40.295360
3334.694257	447687.765999	40.300378
3338.213193	448345.399937	40.305396
3341.702659	449065.434632	40.310413
3344.945524	449750.205085	40.315431
3347.851539	450449.080187	40.320448
3351.253945	451155.043146	40.325466
3354.584533	451854.972834	40.330484
3357.534212	452608.084360	40.335501
3361.233183	453301.888837	40.340519
3364.578968	454042.693304	40.345536
3367.859181	454781.813942	40.350554
3370.814084	455521.872771	40.355572
3374.550905	456256.369038	40.360589
3378.043642	457022.101528	40.365607
3381.007580	457743.210975	40.370624
3384.359483	458529.660242	40.375642
3388.137155	459268.908295	40.380660
3391.240419	460028.223425	40.385677
3394.612754	460802.394928	40.390695
3398.596088	461541.685764	40.395712
3401.763487	462321.805638	40.400730
3405.410442	463095.245163	40.405748
3408.641637	463840.596569	40.410765
3412.390374	464627.370487	40.415783
3415.755310	465379.729183	40.420800
3419.417292	466180.724050	40.425818
3422.938216	466944.130643	40.430836
3426.083885	467697.200630	40.435853
3430.069233	468438.175114	40.440871
3433.708428	469258.022730	40.445888
3436.740794	470028.525468	40.450906
3439.998900	470784.096428	40.455924
3443.942768	471528.254751	40.460941
3447.837654	472341.164145	40.465959
3451.329413	473112.945825	40.470976
3454.408228	473854.021739	40.475994
3458.640422	474625.528149	40.481012
3461.844534	475397.167766	40.486029
3465.086571	476171.855935	40.491047
3468.412459	476925.925294	40.496064
3472.566155	477662.394743	40.501082
3475.605442	478467.358163	40.506100
3478.966726	479232.405637	40.511117
3482.678599	479960.992045	40.516122
3486.008791	480683.756444	40.521127
3489.585523	481337.084365	40.526132
3492.883421	481926.183487	40.531136
3495.741994	482460.205500	40.536141
3498.424851	482971.085140	40.541146
3500.858192	483357.450229	40.546151
3503.305863	483716.496056	40.551156
3505.350322	484029.341092	40.556160
3507.755009	484270.736972	40.561165
3509.696577	484503.691378	40.566170
3511.132725	484690.719882	40.571175
3512.535790	484762.643682	40.576180
3514.125438	484840.769365	40.581184
3515.024829	484918.345195	40.586189
3515.632036	484915.108056	40.591194
3517.077252	484884.126825	40.596199
3517.781298	484847.081710	40.601204
3519.172772	484741.126305	40.606208
3519.823934	484685.191562	40.611213
3519.848532	484562.428046	40.616218
3520.868494	484396.188010	40.621223
3521.267636	484232.628595	40.626228
3521.485099	484088.248158	40.631232
3521.851270	483886.337066	40.636237
3522.319049	483697.631834	40.641242
3522.233146	483469.795818	40.646247
3522.452640	483227.721852	40.651252
3522.429943	483018.921707	40.656256
3522.289895	482812.569985	40.661261
3522.285321	482554.866347	40.666266
3521.787683	482304.331084	40.671271
3521.729222	482046.274568	40.676276
3521.841264	481808.050992	40.681280
3521.299343	481591.818270	40.686285
3521.189677	481304.116838	40.691290
3521.016828	481095.117219	40.696295
3520.877853	480851.195615	40.701300
3520.582816	480583.225153	40.706304
3520.719755	480325.571250	40.711309
3520.637649	480115.330698	40.716314
3520.244849	479858.615923	40.721319
3519.530497	479616.036919	40.726324
3520.065925	479355.722877	40.731328
3519.900182	479131.548678	40.736333
3519.379483	478926.077932	40.741338
3519.167083	478666.633244	40.746343
3518.989756	478413.970798	40.751348
3518.636811	478222.403363	40.756352
3518.130179	477965.986230	40.761357
3518.122426	477764.831739	40.766362
3517.809605	477533.922127	40.771367
3517.712796	477297.400571	40.776372
3517.369140	477128.983383	40.781376
3516.895609	476897.483642	40.786381
3517.143651	476675.852084	40.791386
3516.542460	476507.216964	40.796391
3516.306818	476273.543672	40.801396
3516.345365	476092.436656	40.806400
3515.829394	475874.160948	40.811405
3515.581846	475709.619580	40.816410
3515.697124	475515.063168	40.821415
3515.102724	475331.109484	40.826420
3514.835406	475163.728271	40.831424
3514.851247	474960.261071	40.836429
3514.612425	474831.700359	40.841434
3514.413359	474624.614131	40.846439
3514.112610	474478.877109	40.851444
3513.908167	474294.446880	40.856448
3512.986014	474159.298746	40.861453
3513.250629	473996.436735	40.866458
3513.052026	473847.941721	40.871463
3512.806204	473719.273709	40.876468
3512.900350	473534.029035	40.881472
3512.577383	473425.749765	40.886477
3512.520588	473247.826121	40.891482
3512.259840	473160.066374	40.896487
3511.843654	473014.539919	40.901492
3512.296763	472867.556994	40.906496
3511.552705	472750.824081	40.911501
3511.708091	472597.042516	40.916506
3511.455937	472510.140444	40.921511
3510.749051	472389.445385	40.926516
3511.072997	472233.809430	40.931520
3510.657998	472159.656247	40.936525
3510.360737	472025.054312	40.941530
3510.469407	471921.869912	40.946535
3510.265367	471803.069107	40.951540
3509.945183	471683.018545	40.956544
3509.306401	471599.164865	40.961549
3509.411081	471510.224983	40.966554
3509.564502	471421.226317	40.971559
3509.563180	471341.529454	40.976564
3509.330487	471238.395593	40.981568
3509.246045	471151.562686	40.986573
3508.946604	471077.032461	40.991578
3509.211174	470989.281837	40.996583
3508.855838	470918.714385	41.001588
3509.096443	470837.000083	41.006592
3508.953094	470742.924789	41.011597
3508.772935	470673.089305	41.016602
3508.626168	470596.809438	41.021607
3508.284350	470522.790917	41.026612
3508.319707	470424.731339	41.031616
3507.750108	470393.742082	41.036621
3507.888700	470292.522148	41.041626
3508.063961	470253.049369	41.046631
3508.030469	470174.164317	41.051636
3508.112074	470100.635080	41.056640
3507.938396	470046.209561	41.061645
3507.667202	469993.218947	41.066650
3507.974349	469931.771063	41.071655
3507.374044	469860.275405	41.076660
3507.504098	469814.876857	41.081664
3507.303947	469744.432995	41.086669
3507.342861	469695.854376	41.091674
3507.459270	469652.840625	41.096679
3507.109769	469577.856617	41.101684
3507.627795	469536.198814	41.106688
3507.388035	469474.683916	41.111693
3507.372593	469427.735744	41.116698
3507.243460	469363.211578	41.121703
3507.084107	469318.618233	41.126708
3507.259002	469263.932771	41.131712
3507.158084	469222.879198	41.136717
3507.173322	469163.503316	41.141722
3507.036875	469100.602000	41.146727
3506.694794	469079.969025	41.151732
3507.265772	468991.502418	41.156736
3506.567619	468974.931207	41.161741
3506.913910	468914.082591	41.166746
3506.920683	468871.946528	41.171751
3506.632833	468827.169630	41.176756
3506.475242	468799.459352	41.181760
3506.373983	468751.357031	41.186765
3506.562054	468694.994760	41.191770
3506.435258	468675.493563	41.196775
3506.426279	468623.167894	41.201780
3506.493693	468582.492098	41.206784
3506.375018	468554.471118	41.211789
3506.038041	468496.467336	41.216794
3506.388055	468483.583643	41.221799
3506.329377	468424.572285	41.226804
3506.207129	468399.441851	41.231808
3506.123048	468368.829194	41.236813
3506.045607	468324.372904	41.241818
3505.980316	468301.870025	41.246823
3505.865509	468267.357765	41.251828
3506.036059	468222.405715	41.256832
3505.717539	468213.379728	41.261837
3505.744335	468184.422563	41.266842
3505.798367	468136.902758	41.271847
3505.588744	468113.611198	41.276852
3505.471401	468086.096441	41.281856
3505.389539	468079.872521	41.286861
3505.975687	468040.939103	41.291866
3505.778722	468021.803330	41.296871
3505.201897	468011.246194	41.301876
3505.789131	467965.619267	41.306880
3505.462956	467935.399186	41.311885
3505.623124	467933.294880	41.316890
3505.149517	467908.878572	41.321895
3505.423712	467846.263541	41.326900
3505.595927	467861.853866	41.331904
3505.184176	467843.360354	41.336909
3505.343480	467795.265370	41.341914
3505.288810	467788.834240	41.346919
3505.116853	467770.911244	41.351924
3505.735024	467740.845870	41.356928
3505.308375	467726.005492	41.361933
3504.831030	467699.054194	41.366938
3504.968905	467685.950010	41.371943
3504.863773	467687.234261	41.376948
3504.966292	467655.171283	41.381952
3504.958715	467637.932091	41.386957
3505.242020	467635.301225	41.391962
3505.348265	467599.485259	41.396967
3505.253808	467600.362172	41.401972
3505.451468	467574.875949	41.406976
3505.403388	467559.722085	41.411981
3505.196499	467525.983771	41.416986
3505.280788	467523.435052	41.421991
3504.785465	467500.390797	41.426996
3505.314606	467478.452284	41.432000
3504.892201	467479.888107	41.437005
3505.028856	467457.910191	41.442010
3505.113122	467427.016021	41.447015
3504.676840	467445.694567	41.452020
3505.093637	467402.882269	41.457024
3504.668419	467394.075623	41.462029
3504.693242	467402.793358	41.467034
3504.954068	467359.802794	41.472039
3504.900120	467371.828986	41.477044
3505.639948	467350.414824	41.482048
3505.147022	467327.522124	41.487053
3504.780991	467326.160125	41.492058
3505.479935	467291.010576	41.497063
3504.983154	467270.805935	41.502068
3505.044018	467252.034376	41.507072
3504.896092	467243.741628	41.512077
3505.369963	467222.927159	41.517082
3505.063458	467217.144152	41.522087
3504.944098	467190.794828	41.527092
3505.030895	467190.121871	41.532096
3504.835243	467177.830705	41.537101
3504.652406	467137.293089	41.542106
3504.914868	467147.950987	41.547111
3505.010037	467123.241041	41.552116
3505.074703	467108.170450	41.557120
3505.004106	467104.429164	41.562125
3505.078423	467070.949927	41.567130
3505.377172	467075.821380	41.572135
3504.769549	467049.498341	41.577140
3504.934416	467040.902535	41.582144
3504.576331	467013.627261	41.587149
3504.731444	467019.180638	41.592154
3504.874359	467002.221392	41.597159
3504.853972	466981.687639	41.602164
3504.885793	466964.036002	41.607168
3505.118434	466969.425013	41.612173
3505.161200	466945.280935	41.617178
3504.854432	466918.453806	41.622183
3504.526780	466933.363191	41.627188
3505.043931	466906.253700	41.632192
3504.911340	466887.968772	41.637197
3504.593469	466885.534247	41.642202
3504.787636	466883.627300	41.647207
3504.767891	466855.182754	41.652212
3504.826549	466834.078568	41.657216
3504.437631	466835.864102	41.662221
3504.445768	466809.950533	41.667226
3504.555803	466806.231354	41.672231
3504.407457	466833.891119	41.677236
3504.918667	466800.646657	41.682240
3504.496282	466786.920540	41.687245
3504.668908	466808.190984	41.692250
3505.017773	466783.795508	41.697255
3504.646401	466776.653490	41.702260
3504.763747	466772.578186	41.707264
3504.805679	466754.113432	41.712269
3504.760547	466718.725573	41.717274
3505.385220	466715.381423	41.722279
3504.896588	466703.643379	41.727284
3504.770447	466683.785270	41.732288
3505.084231	466673.441664	41.737293
3504.863682	466667.340666	41.742298
3505.198741	466648.728072	41.747303
3504.850057	466638.742699	41.752308
3505.042804	466593.580840	41.757312
3504.720619	466616.603093	41.762317
3504.845780	466605.731463	41.767322
3504.565403	466579.913922	41.772327
3504.868428	466540.464690	41.777332
3505.026807	466554.942556	41.782336
3504.908197	466523.673458	41.787341
3504.502922	466542.043639	41.792346
3505.101488	466497.527369	41.797351
3504.692262	466507.378977	41.802356
3505.010231	466470.513446	41.807360
3504.777844	466464.059292	41.812365
3504.870887	466457.705830	41.817370
3505.108831	466445.599258	41.822375
3504.441605	466427.601271	41.827380
3504.818151	466406.040737	41.832384
3504.897877	466408.512886	41.837389
3504.950079	466361.242930	41.842394
3504.547583	466389.906931	41.847399
3504.344668	466374.117461	41.852404
3504.788783	466372.525934	41.857408
3504.610626	466372.199086	41.862413
3504.657177	466336.643970	41.867418
3504.747426	466343.982628	41.872423
3504.597720	466345.324715	41.877428
3504.609605	466299.227324	41.882432
3504.763315	466305.643183	41.887437
3504.676410	466319.044354	41.892442
3504.616543	466273.820320	41.897447
3504.618824	466281.375744	41.902452
3504.642430	466275.540305	41.907456
3504.317018	466258.045962	41.912461
3504.677077	466252.005209	41.917466
3504.982052	466241.764207	41.922471
3504.435850	466247.885022	41.927476
3504.766262	466219.282862	41.932480
3504.579212	466214.139934	41.937485
3504.416518	466220.656536	41.942490
3504.479016	466196.254936	41.947495
3504.470915	466181.702293	41.952500
3504.373442	466188.411439	41.957504
3504.651140	466183.550023	41.962509
3504.532873	466169.420466	41.967514
3504.886320	466139.343954	41.972519
3504.647065	466150.233784	41.977524
3504.775546	466147.576496	41.982528
3504.770668	466130.031387	41.987533
3504.683602	466126.647504	41.992538
3504.806977	466112.175454	41.997543
3504.581619	466090.659022	42.002548
3504.709288	466081.663022	42.007552
3504.027458	466089.580191	42.012557
3504.107819	466066.494096	42.017562
3504.539655	466062.064688	42.022567
3504.720321	466054.125225	42.027572
3504.611479	466049.679847	42.032576
3504.587344	466059.420087	42.037581
3504.759250	466017.455073	42.042586
3504.379602	466020.963376	42.047591
3504.326221	466027.716315	42.052596
3504.849260	466011.862549	42.057600
3504.795734	466002.438756	42.062605
3504.719542	465993.931336	42.067610
3504.698063	465981.358394	42.072615
3504.626483	465948.204712	42.077620
3504.854231	465962.266330	42.082624
3504.901919	465945.169159	42.087629
3504.759804	465927.442730	42.092634
3504.985334	465922.792344	42.097639
3504.658410	465904.435861	42.102644
3504.995532	465890.893389	42.107648
3504.873325	465894.716002	42.112653
3504.764096	465866.892810	42.117658
3504.854026	465865.255803	42.122663
3504.647956	465846.677324	42.127668
3504.766630	465824.193446	42.132672
3504.787904	465813.692810	42.137677
3504.594669	465810.984904	42.142682
3504.892505	465803.990345	42.147687
3504.784812	465775.101852	42.152692
3504.974167	465777.962438	42.157696
3504.679962	465759.854216	42.162701
3504.595303	465743.994875	42.167706
3504.552028	465716.516043	42.172711
3504.601674	465736.184229	42.177716
3504.608231	465705.096990	42.182720
3504.513647	465744.007639	42.187725
3504.440948	465687.323591	42.192730
3504.275645	465692.116572	42.197735
3504.161773	465693.402324	42.202740
3504.531952	465668.241528	42.207744
3504.205175	465690.656967	42.212749
3504.468188	465685.341355	42.217754
3504.466978	465661.608463	42.222759
3504.891756	465656.520835	42.227764
3504.841177	465671.640870	42.232768
3504.502635	465627.372317	42.237773
3504.616137	465617.769819	42.242778
3504.403721	465629.619196	42.247783
3504.461946	465613.585040	42.252788
3504.438126	465598.882347	42.257792
3504.845006	465588.117808	42.262797
3504.403835	465600.966880	42.267802
3504.660938	465580.641475	42.272807
3504.538758	465556.674026	42.277812
3504.699366	465546.962627	42.282816
3504.595717	465557.983462	42.287821
3504.318965	465519.739637	42.292826
3504.656997	465522.475335	42.297831
3504.780114	465520.376649	42.302836
3504.690942	465489.912770	42.307840
3504.740661	465502.532180	42.312845
3504.444941	465474.737951	42.317850
3504.432025	465505.319340	42.322855
3504.473782	465469.459261	42.327860
3504.205089	465470.718784	42.332864
3504.382359	465467.293018	42.337869
3504.740490	465464.802198	42.342874
3504.487156	465468.645612	42.347879
3504.311400	465428.103613	42.352884
3504.624797	465433.480253	42.357888
3504.671107	465439.913348	42.362893
3504.304438	465411.775265	42.367898
3504.740781	465398.622497	42.372903
3504.713941	465391.019858	42.377908
3504.574986	465379.225813	42.382912
3504.538295	465399.161517	42.387917
3504.420390	465342.230135	42.392922
3504.794419	465360.427451	42.397927
3504.662210	465357.963404	42.402932
3504.240839	465360.362736	42.407936
3504.634669	465333.422874	42.412941
3504.105579	465347.046681	42.417946
3504.943081	465328.353526	42.422951
3504.774684	465312.608524	42.427956
3504.724498	465305.060257	42.432960
3504.918832	465302.899581	42.437965
3504.199451	465282.576088	42.442970
3504.791238	465257.785485	42.447975
3504.127749	465263.772978	42.452980
3504.545718	465272.784439	42.457984
3504.964056	465221.954919	42.462989
3504.451329	465261.236811	42.467994
3504.484125	465226.341281	42.472999
3504.651727	465201.617655	42.478004
3504.605537	465218.917965	42.483008
3504.384395	465221.285666	42.488013
3504.123720	465195.260479	42.493018
3504.506799	465195.960589	42.498023
3504.034556	465180.212800	42.503028
3504.660834	465152.982409	42.508032
3504.384936	465182.185864	42.513037
3504.332804	465164.343152	42.518042
3504.691059	465174.276923	42.523047
3504.673567	465164.492075	42.528052
3504.794793	465135.617248	42.533056
3504.552294	465131.243516	42.538061
3504.733538	465134.409749	42.543066
3504.945527	465091.625173	42.548071
3504.206000	465115.069998	42.553076
3504.609376	465091.323240	42.558080
3504.672499	465069.760182	42.563085
3504.563818	465072.008699	42.568090
3504.599740	465053.188429	42.573095
3504.582576	465049.844040	42.578100
3504.364517	465041.865794	42.583104
3504.708190	465020.917617	42.588109
3504.455090	465034.498002	42.593114
3504.703914	465010.319163	42.598119
3504.057478	465001.191489	42.603124
3504.620012	464994.864816	42.608128
3504.710457	464988.663468	42.613133
3504.219217	464972.056402	42.618138
3504.453182	464969.128730	42.623143
3504.486424	464949.953799	42.628148
3504.840296	464970.943868	42.633152
3504.698776	464944.747403	42.638157
3504.583985	464932.290017	42.643162
3504.455191	464914.560640	42.648167
3503.732669	464942.516462	42.653172
3504.410188	464918.371190	42.658176
3504.406850	464923.088031	42.663181
3504.416925	464905.590265	42.668186
3504.086392	464901.534680	42.673191
3503.995267	464902.411176	42.678196
3504.090410	464895.397643	42.683200
3504.362884	464898.448065	42.688205
3503.919628	464908.153645	42.693210
3504.431269	464898.842893	42.698215
3504.252716	464873.260756	42.703220
3504.183556	464883.110076	42.708224
3504.495836	464849.184028	42.713229
3504.323533	464890.441340	42.718234
3504.178123	464862.571844	42.723239
3504.167428	464896.095139	42.728244
3504.504533	464867.439399	42.733248
3504.448704	464840.062851	42.738253
3504.037043	464856.761939	42.743258
3504.551553	464826.708838	42.748263
3504.281818	464845.312623	42.753268
3504.191175	464856.179622	42.758272
3504.256747	464834.058090	42.763277
3504.634006	464803.215232	42.768282
3504.133722	464846.350159	42.773287
3503.837661	464821.597950	42.778292
3504.467742	464821.396902	42.783296
3504.242471	464833.806601	42.788301
3504.317862	464827.709013	42.793306
3504.480759	464800.652840	42.798311
3504.202539	464812.563783	42.803316
3504.476530	464800.704151	42.808321
3504.796472	464795.531463	42.813325
3504.181904	464787.311509	42.818330
3504.119734	464758.820156	42.823335
3504.344035	464772.426681	42.828340
3504.203386	464769.507475	42.833345
3504.404986	464765.164905	42.838349
3503.714240	464767.049025	42.843354
3504.615230	464767.565866	42.848359
3504.069840	464756.697849	42.853364
3504.113237	464742.947506	42.858369
3504.447374	464735.186153	42.863373
3504.230042	464738.719724	42.868378
3504.508993	464737.002043	42.873383
3504.510666	464742.326698	42.878388
3504.289860	464734.095201	42.883393
3504.316175	464705.234796	42.888397
3504.141529	464696.438136	42.893402
3504.167891	464717.328075	42.898407
3504.532852	464698.810486	42.903412
3504.109497	464702.325911	42.908417
3504.486138	464710.887716	42.913421
3504.672190	464671.453519	42.918426
3504.472658	464679.548547	42.923431
3504.418763	464680.774166	42.928436
3504.463405	464653.787212	42.933441
3504.397982	464651.667526	42.938445
3503.943597	464663.099254	42.943450
3504.506760	464638.160317	42.948455
3504.640253	464659.439093	42.953460
3504.445889	464626.911335	42.958465
3504.251142	464618.929246	42.963469
3504.510755	464623.807450	42.968474
3504.275913	464605.942436	42.973479
3504.163494	464615.748001	42.978484
3503.985625	464599.851829	42.983489
3504.437206	464614.690387	42.988493
3504.068769	464598.063621	42.993498
3503.881011	464586.428993	42.998503
3503.934285	464586.724823	43.003508
3503.974123	464586.566349	43.008513
3504.082022	464593.649249	43.013517
3504.351803	464585.644443	43.018522
3504.617792	464581.494516	43.023527
3504.249648	464595.955502	43.028532
3504.220998	464596.771422	43.033537
3504.613888	464552.334324	43.038541
3504.252532	464577.951393	43.043546
3504.439592	464550.231800	43.048551
3504.332249	464556.131589	43.053556
3504.028808	464552.020940	43.058561
3504.337243	464551.667870	43.063565
3503.816290	464528.370867	43.068570
3504.101755	464535.070721	43.073575
3504.017663	464519.616097	43.078580
3504.226959	464548.388729	43.083585
3504.304062	464513.840035	43.088589
3504.299078	464556.998690	43.093594
3504.242699	464529.824690	43.098599
3504.231391	464537.788593	43.103604
3504.509843	464516.647375	43.108609
3504.902202	464510.854601	43.113613
3504.466229	464488.710554	43.118618
3504.100530	464513.973384	43.123623
3504.281419	464489.297551	43.128628
3504.451007	464467.869204	43.133633
3504.727177	464461.536921	43.138637
3504.172093	464476.078249	43.143642
3504.555278	464469.678340	43.148647
3504.253273	464440.058037	43.153652
3504.045730	464429.390028	43.158657
3504.317892	464441.112758	43.163661
3504.159633	464431.451252	43.168666
3504.394316	464432.479131	43.173671
3504.175264	464442.403058	43.178676
3504.485579	464427.849609	43.183681
3504.436833	464403.615688	43.188685
3504.436379	464402.702861	43.193690
3504.497325	464409.032523	43.198695
3504.454425	464384.138367	43.203700
3504.083208	464391.905635	43.208705
3504.311656	464365.802132	43.213709
3504.336091	464361.233908	43.218714
3504.550960	464372.103581	43.223719
3504.617126	464366.108749	43.228724
3503.872295	464359.126370	43.233729
3504.190744	464371.348971	43.238733
3504.242215	464348.519161	43.243738
3504.152766	464326.675182	43.248743
3504.505882	464353.853184	43.253748
3504.554922	464355.518985	43.258753
3504.562527	464334.826113	43.263757
3504.305477	464325.383033	43.268762
3504.626602	464324.723665	43.273767
3504.384027	464318.574758	43.278772
3504.313137	464308.341524	43.283777
3504.887790	464288.066134	43.288781
3504.380003	464290.225667	43.293786
3504.565615	464281.726902	43.298791
3504.136429	464272.006714	43.303796
3504.211597	464282.644938	43.308801
3503.986882	464258.895100	43.313805
3504.035005	464251.229494	43.318810
3504.255549	464238.363700	43.323815
3504.286404	464245.509607	43.328820
3503.942560	464238.920247	43.333825
3504.486632	464245.427175	43.338829
3504.128748	464249.388760	43.343834
3504.335165	464243.422442	43.348839
3504.079981	464219.170226	43.353844
3504.226059	464216.966354	43.358849
3504.314999	464217.459413	43.363853
3504.119909	464227.024646	43.368858
3504.041417	464219.480470	43.373863
3504.089987	464217.444154	43.378868
3504.325398	464219.891951	43.383873
3504.628371	464224.661963	43.388877
3504.129032	464191.319590	43.393882
3504.126142	464191.573587	43.398887
3504.087558	464204.917730	43.403892
3504.038035	464188.798107	43.408897
3504.310953	464188.653507	43.413901
3504.017733	464199.958577	43.418906
3504.397490	464202.535707	43.423911
3504.273888	464195.860810	43.428916
3503.996273	464182.262274	43.433921
3504.466843	464165.806858	43.438925
3504.394224	464164.499704	43.443930
3504.763736	464173.772864	43.448935
3504.414991	464178.392315	43.453940
3504.204528	464135.571172	43.458945
3504.231904	464142.311941	43.463949
3504.121511	464144.002957	43.468954
3504.382654	464130.167092	43.473959
3504.436371	464127.267794	43.478964
3504.447396	464129.142482	43.483969
3504.264705	464116.137485	43.488973
3504.209751	464110.770310	43.493978
3504.607585	464085.958296	43.498983
3504.419206	464090.400273	43.503988
3504.106576	464105.258537	43.508993
3504.540880	464079.426444	43.513997
3504.102412	464086.291574	43.519002
3504.483467	464050.324779	43.524007
3504.469909	464054.130548	43.529012
3504.409965	464066.413128	43.534017
3504.488938	464054.888201	43.539021
3504.229961	464019.986108	43.544026
3504.143855	464033.439299	43.549031
3504.454602	464009.401694	43.554036
3504.252154	464047.774600	43.559041
3504.390083	464003.680959	43.564045
3504.076247	464030.457627	43.569050
3504.239163	463988.236479	43.574055
3504.316633	464016.827796	43.579060
3504.079805	463995.666075	43.584065
3504.393462	463987.400535	43.589069
3504.373712	464005.001939	43.594074
3503.898186	464009.996472	43.599079
3504.576052	463996.043942	43.604084
3504.127202	463976.386465	43.609089
3504.768828	463974.459257	43.614093
3504.234528	463973.275776	43.619098
3504.701509	463954.690708	43.624103
3504.514496	463978.505884	43.629108
3504.021158	463933.548274	43.634113
3504.079320	463955.448243	43.639117
3504.532037	463935.141078	43.644122
3504.067854	463934.301524	43.649127
3504.228980	463947.766409	43.654132
3503.919520	463941.425102	43.659137
3504.568962	463922.608305	43.664141
3504.207876	463908.718494	43.669146
3504.250803	463915.862603	43.674151
3504.761093	463902.291508	43.679156
3504.124680	463908.883684	43.684161
3504.374587	463893.781547	43.689165
3504.062541	463893.881547	43.694170
3504.295772	463876.296957	43.699175
3504.179218	463868.403662	43.704180
3503.885651	463884.019804	43.709185
3504.410014	463878.763873	43.714189
3503.939598	463879.801789	43.719194
3504.262736	463879.243522	43.724199
3503.931539	463874.934266	43.729204
3503.916467	463887.970594	43.734209
3504.038373	463874.460867	43.739213
3503.949302	463849.522672	43.744218
3504.419295	463855.382120	43.749223
3504.433745	463853.959755	43.754228
3503.824879	463844.673499	43.759233
3503.925265	463852.417139	43.764237
3503.847672	463854.863732	43.769242
3503.910142	463853.839505	43.774247
3504.318771	463861.230128	43.779252
3504.278194	463868.133871	43.784257
3504.511751	463848.165559	43.789261
3504.078298	463839.865895	43.794266
3504.184828	463833.255944	43.799271
3503.855982	463818.448091	43.804276
3503.972257	463834.912382	43.809281
3504.123186	463816.529295	43.814285
3503.970628	463839.223428	43.819290
3504.229291	463839.233226	43.824295
3504.172754	463809.776121	43.829300
3504.362778	463845.044394	43.834305
3504.179849	463833.662175	43.839309
3504.446061	463798.270988	43.844314
3504.494850	463795.270992	43.849319
3504.622336	463825.021129	43.854324
3504.524755	463795.316911	43.859329
3504.538988	463803.682778	43.864333
3504.489738	463771.384369	43.869338
3504.363583	463756.595154	43.874343
3504.315624	463765.224447	43.879348
3504.241962	463776.850050	43.884353
3504.168239	463762.711862	43.889357
3504.280502	463730.387864	43.894362
3504.322030	463732.714212	43.899367
3504.530214	463731.007637	43.904372
3504.052001	463723.678612	43.909377
3504.322573	463722.672203	43.914381
3504.054851	463732.553433	43.919386
3504.333073	463714.910884	43.924391
3504.338937	463692.442601	43.929396
3504.030053	463692.795682	43.934401
3504.358352	463687.570693	43.939405
3504.381841	463701.463217	43.944410
3504.455960	463682.787859	43.949415
3504.094649	463666.717123	43.954420
3503.757902	463688.476914	43.959425
3503.784207	463653.326271	43.964429
3504.216127	463671.465157	43.969434
3504.085676	463671.384307	43.974439
3503.965422	463659.637075	43.979444
3504.111973	463669.960021	43.984449
3504.429664	463665.041001	43.989453
3504.108436	463681.574557	43.994458
3504.188543	463669.592798	43.999463
3504.369828	463670.172707	44.004468
3504.118106	463665.901563	44.009473
3504.470635	463630.902190	44.014477
3504.421003	463646.479950	44.019482
3504.464175	463640.640700	44.024487
3504.651777	463629.757691	44.029492
3503.900292	463636.013121	44.034497
3504.510468	463612.992795	44.039501
3504.043030	463605.104144	44.044506
3504.579963	463614.858251	44.049511
3504.385186	463586.741319	44.054516
3504.022199	463622.401660	44.059521
3504.172315	463593.266613	44.064525
3504.290998	463597.254428	44.069530
3504.354953	463575.689739	44.074535
3504.155708	463578.307741	44.079540
3504.158582	463587.486953	44.084545
3504.432415	463577.756770	44.089549
3504.297642	463589.899299	44.094554
3504.352828	463557.026180	44.099559
3504.717344	463551.795434	44.104564
3504.336984	463550.080431	44.109569
3504.373888	463546.169380	44.114573
3504.526000	463532.299647	44.119578
3504.746235	463507.920772	44.124583
3504.406928	463503.917023	44.129588
3504.206219	463506.230965	44.134593
3504.455379	463490.367913	44.139597
3504.157476	463488.589156	44.144602
3504.127680	463469.067850	44.149607
3504.583221	463455.200828	44.154612
3504.199059	463469.969401	44.159617
3504.512680	463481.939688	44.164621
3504.223380	463452.620317	44.169626
3504.553517	463450.285842	44.174631
3504.274793	463439.628592	44.179636
3504.361124	463438.397705	44.184641
3504.438502	463406.585905	44.189645
3504.046919	463448.996412	44.194650
3504.173395	463394.506369	44.199655
3504.550858	463405.604418	44.204660
3504.124469	463386.602173	44.209665
3504.198474	463410.985326	44.214669
3504.115935	463389.392888	44.219674
3504.304398	463408.736966	44.224679
3503.931815	463392.718524	44.229684
3503.848431	463432.950237	44.234689
3504.307086	463389.768271	44.239693
3504.446749	463393.499222	44.244698
3504.223585	463364.879317	44.249703
3504.589146	463370.045364	44.254708
3504.248700	463348.848668	44.259713
3504.364506	463380.528515	44.264717
3504.186174	463349.568519	44.269722
3503.998435	463347.366602	44.274727
3504.339838	463356.340256	44.279732
3503.742292	463353.239485	44.284737
3504.456219	463330.050308	44.289741
3503.965485	463366.289152	44.294746
3504.151166	463337.503158	44.299751
3504.390367	463341.776275	44.304756
3503.911310	463357.168529	44.309761
3504.407273	463345.120863	44.314765
3504.003315	463325.557130	44.319770
3504.221724	463308.988765	44.324775
3504.386116	463331.379751	44.329780
3504.172342	463297.990858	44.334785
3504.790587	463306.261453	44.339789
3504.361374	463314.241142	44.344794
3504.409268	463266.559302	44.349799
3504.577169	463294.985131	44.354804
3504.082990	463272.747595	44.359809
3504.351659	463277.776827	44.364813
3504.133224	463282.984479	44.369818
3504.672238	463220.212592	44.374823
3504.524547	463260.759093	44.379828
3503.989520	463239.238020	44.384833
3504.472629	463251.080213	44.389837
3504.387222	463235.726309	44.394842
3504.147033	463233.532670	44.399847
3504.156946	463215.019207	44.404852
3504.166134	463203.910595	44.409857
3504.807337	463217.756518	44.414861
3504.127051	463200.011455	44.419866
3504.090815	463223.042873	44.424871
3504.240266	463208.159004	44.429876
3504.187139	463184.888037	44.434881
3504.455689	463176.223576	44.439885
3504.545743	463176.919353	44.444890
3504.266821	463175.391158	44.449895
3504.379162	463173.851841	44.454900
3504.504543	463162.014797	44.459905
3504.124522	463154.112164	44.464909
3504.259851	463130.354894	44.469914
3504.654977	463137.392877	44.474919
3504.651504	463137.900567	44.479924
3503.931547	463113.416257	44.484929
3504.497484	463108.863618	44.489933
3504.351837	463078.202373	44.494938
3504.512163	463106.122471	44.499943
3504.568057	463085.420768	44.504948
3504.224977	463070.107472	44.509953
3504.179199	463059.666805	44.514957
3504.325525	463057.716366	44.519962
3504.026227	463059.944501	44.524967
3504.388687	463066.024032	44.529972
3504.182725	463056.115859	44.534977
3504.306181	463071.159499	44.539981
3504.052151	463026.872222	44.544986
3503.923272	463034.500238	44.549991
3504.260632	463013.652545	44.554996
3503.917663	463014.568921	44.560001
3504.157482	463041.867923	44.565005
3504.074745	463024.991912	44.570010
3504.240470	463027.704449	44.575015
3504.428712	463014.589443	44.580020
3503.986850	463040.474649	44.585025
3504.111220	463027.014720	44.590029
3504.712902	462999.836218	44.595034
3504.225185	462986.726595	44.600039
3504.386733	463003.336519	44.605044
3504.003412	463011.156912	44.610049
3504.489950	462989.423413	44.615053
3504.366026	462975.039054	44.620058
3504.116300	462971.528226	44.625063
3504.260912	462950.102320	44.630068
3503.983209	462971.954935	44.635073
3504.299426	462969.267584	44.640077
3504.148606	462951.489351	44.645082
3504.059397	462986.042391	44.650087
3504.239525	462945.490178	44.655092
3504.108241	462974.420179	44.660097
3504.663833	462923.107077	44.665101
3504.129659	462948.854829	44.670106
3504.487353	462907.919454	44.675111
3504.673371	462941.059675	44.680116
3504.335374	462914.891791	44.685121
3504.339156	462906.928407	44.690125
3504.073264	462888.813283	44.695130
3504.123584	462886.015792	44.700135
3504.283003	462906.480712	44.705140
3504.191717	462896.250031	44.710145
3504.355010	462894.449050	44.715149
3504.167106	462882.407778	44.720154
3503.850738	462875.813656	44.725159
3504.184958	462867.290848	44.730164
3503.808377	462866.792430	44.735169
3503.984831	462877.212466	44.740173
3503.809055	462844.273331	44.745178
3503.831251	462860.753234	44.750183
3503.487962	462858.372978	44.755188
3503.603979	462862.614942	44.760193
3503.574598	462867.691377	44.765197
3503.787998	462907.268541	44.770202
3503.765243	462893.476755	44.775207
3504.409641	462911.937726	44.780212
3503.914139	462892.337350	44.785217
3503.919199	462885.590993	44.790221
3503.808871	462878.355688	44.795226
3503.806678	462869.987488	44.800231
3503.742079	462884.908825	44.805236
3504.328818	462878.476276	44.810241
3504.188958	462869.318342	44.815245
3504.026561	462886.740330	44.820250
3504.045097	462887.954602	44.825255
3503.776681	462877.447598	44.830260
3504.242528	462897.154040	44.835265
3504.009362	462876.751415	44.840269
3503.918993	462890.358147	44.845274
3503.815811	462877.339835	44.850279
3504.240857	462874.990300	44.855284
3504.004085	462905.458613	44.860289
3503.978237	462885.631847	44.865293
3504.332984	462878.170882	44.870298
3503.760913	462894.491093	44.875303
3504.173070	462849.235952	44.880308
3504.056691	462863.151122	44.885313
3503.928562	462865.859406	44.890317
3503.906565	462844.611882	44.895322
3503.712007	462869.139530	44.900327
3503.744454	462858.737121	44.905332
3503.734416	462860.361657	44.910337
3503.682525	462855.399431	44.915341
3504.223512	462881.078768	44.920346
3504.084884	462862.487044	44.925351
3504.568495	462859.063167	44.930356
3504.104031	462887.031578	44.935361
3504.467196	462852.942193	44.940365
3504.162475	462882.305475	44.945370
3504.244613	462846.434640	44.950375
3503.853331	462869.471831	44.955380
3503.830881	462853.955551	44.960385
3504.037651	462861.327705	44.965389
3504.278338	462834.966826	44.970394
3503.870281	462874.591554	44.975399
3503.919590	462836.747879	44.980404
3503.883541	462863.279215	44.985409
3503.631688	462844.705371	44.990413
3503.856365	462835.033342	44.995418
3503.645056	462874.221227	45.000423
3504.061147	462851.382923	45.005428
3503.785442	462863.903161	45.010433
3504.021277	462868.227623	45.015437
3504.288767	462852.969826	45.020442
3503.758441	462859.646987	45.025447
3504.129941	462875.361615	45.030452
3504.056255	462869.997091	45.035457
3503.794807	462866.589536	45.040461
3503.918780	462866.975653	45.045466
3503.824328	462876.677732	45.050471
3503.944030	462869.659659	45.055476
3503.977376	462873.661095	45.060481
3504.124711	462868.920975	45.065485
3504.238738	462875.547009	45.070490
3503.934763	462886.753028	45.075495
3504.115431	462873.131951	45.080500
3503.925937	462872.958992	45.085505
3503.993079	462849.719373	45.090509
3504.141610	462845.689116	45.095514
3503.830427	462832.500779	45.100519
3503.943787	462834.460842	45.105524
3503.832401	462872.973598	45.110529
3503.769779	462841.385967	45.115533
3504.153903	462846.802798	45.120538
3503.970669	462851.649962	45.125543
3504.320120	462844.646287	45.130548
3504.191769	462843.905763	45.135553
3504.057178	462837.485772	45.140557
3504.279553	462853.376141	45.145562
3504.255486	462852.923445	45.150567
3503.818374	462839.450706	45.155572
3503.997661	462849.363124	45.160577
3504.219314	462819.049206	45.165581
3504.434875	462831.390381	45.170586
3504.384379	462807.915719	45.175591
3504.457501	462812.823811	45.180596
3504.267437	462828.018609	45.185601
3503.851452	462805.869669	45.190605
3504.260839	462824.722887	45.195610
3504.078076	462789.756039	45.200615
3504.291566	462774.963188	45.205620
3503.824508	462797.403810	45.210625
3504.177131	462778.024312	45.215629
3504.462853	462767.936858	45.220634
3504.055530	462802.033285	45.225639
3503.998489	462793.521569	45.230644
3504.506671	462777.464901	45.235649
3504.114960	462779.707670	45.240653
3504.515627	462744.293507	45.245658
3504.143544	462776.710692	45.250663
3503.930609	462760.970859	45.255668
3504.010704	462738.286977	45.260673
3504.270378	462763.250139	45.265677
3504.160082	462780.562540	45.270682
3503.926661	462771.267197	45.275687
3503.785978	462745.067922	45.280692
3503.726767	462742.997784	45.285697
3504.143752	462793.853213	45.290701
3503.956270	462803.874339	45.295706
3503.710445	462784.995180	45.300711
3504.077627	462744.818775	45.305716
3504.126869	462784.016361	45.310721
3503.977985	462774.656939	45.315725
3504.071708	462725.647983	45.320730
3504.243809	462723.744158	45.325735
3503.647888	462756.653218	45.330740
3504.021967	462710.440154	45.335745
3504.237838	462738.706978	45.340749
3503.533729	462735.622958	45.345754
3503.877403	462713.404576	45.350759
3504.154604	462721.272833	45.355764
3503.935328	462762.440205	45.360769
3503.725847	462740.207841	45.365773
3503.689562	462733.670844	45.370778
3503.681631	462737.780267	45.375783
3503.939572	462743.927128	45.380788
3503.919670	462766.804293	45.385793
3503.975052	462730.481028	45.390797
3504.090045	462751.409583	45.395802
3503.759525	462763.735669	45.400807
3504.452560	462719.855983	45.405812
3503.895962	462763.815471	45.410817
3504.258585	462727.392923	45.415821
3504.110878	462748.413719	45.420826
3503.853521	462760.880399	45.425831
3504.162800	462742.217779	45.430836
3504.073393	462756.889532	45.435841
3504.435687	462753.129784	45.440845
3504.373718	462730.011880	45.445850
3504.168027	462728.522796	45.450855
3504.331248	462728.091215	45.455860
3504.037698	462734.223805	45.460865
3503.980816	462713.488852	45.465869
3504.402484	462729.499970	45.470874
3504.359450	462710.487258	45.475879
3504.293617	462678.088398	45.480884
3504.457080	462684.858832	45.485889
3504.484376	462680.999862	45.490893
3504.642914	462681.989143	45.495898
3504.341312	462661.850725	45.500903
3504.722832	462645.357510	45.505908
3504.732757	462647.638251	45.510913
3504.417233	462632.827478	45.515917
3504.237234	462626.465320	45.520922
3503.859885	462602.534906	45.525927
3504.578417	462586.241976	45.530932
3504.438367	462583.677410	45.535937
3504.529844	462620.687702	45.540941
3504.196811	462598.981909	45.545946
3504.200554	462554.500768	45.550951
3504.456163	462584.993147	45.555956
3503.999777	462583.695833	45.560961
3504.341519	462542.965167	45.565965
3504.522668	462572.759266	45.570970
3504.307666	462572.133865	45.575975
3504.753894	462535.799220	45.580980
3504.336341	462552.602455	45.585985
3504.692745	462499.747546	45.590989
3504.696053	462537.279107	45.595994
3504.074106	462507.453119	45.600999
3504.492759	462504.698802	45.606004
3504.258787	462505.699409	45.611009
3504.138862	462485.887147	45.616013
3504.547586	462513.312278	45.621018
3504.404456	462481.990442	45.626023
3504.299398	462448.481617	45.631028
3504.323083	462482.256828	45.636033
3504.267945	462453.203406	45.641037
3504.153636	462446.323621	45.646042
3503.961394	462455.990625	45.651047
3503.975321	462466.081512	45.656052
3504.024205	462411.854854	45.661057
3503.884506	462442.815667	45.666061
3504.074502	462408.752955	45.671066
3504.141354	462425.682605	45.676071
3504.073978	462415.802953	45.681076
3503.966679	462442.447503	45.686081
3503.650574	462413.384555	45.691085
3503.961483	462442.701849	45.696090
3503.477653	462438.213550	45.701095
3504.030034	462423.924811	45.706100
3503.707214	462453.595849	45.711105
3504.284520	462411.001811	45.716109
3504.311698	462460.296615	45.721114
3503.961609	462440.469969	45.726119
3504.256994	462409.433756	45.731124
3504.155050	462471.479491	45.736129
3503.987093	462440.567273	45.741133
3504.573651	462404.768142	45.746138
3504.153328	462423.245653	45.751143
3504.427013	462384.097744	45.756148
3504.065623	462415.448670	45.761153
3504.244345	462377.025828	45.766157
3504.004536	462413.987394	45.771162
3503.891509	462388.138351	45.776167
3504.076148	462410.121335	45.781172
3503.641755	462410.189956	45.786177
3503.982242	462385.232899	45.791181
3504.221179	462426.480645	45.796186
3503.758942	462427.111579	45.801191
3503.411962	462413.928644	45.806196
3503.921098	462381.286308	45.811201
3504.035257	462431.226782	45.816205
3504.046869	462412.661645	45.821210
3504.007112	462427.782248	45.826215
3503.877541	462404.928278	45.831220
3504.235295	462408.675650	45.836225
3503.941940	462425.865109	45.841229
3504.233980	462375.302438	45.846234
3503.897835	462391.737895	45.851239
3504.056469	462398.255586	45.856244
3504.150325	462378.054401	45.861249
3504.031390	462404.041485	45.866253
3504.282333	462416.377305	45.871258
3503.969368	462393.907345	45.876263
3504.172917	462403.004623	45.881268
3503.845912	462405.592238	45.886273
3504.092369	462376.795363	45.891277
3504.419442	462407.479575	45.896282
3503.968219	462387.009513	45.901287
3504.303392	462348.663332	45.906292
3503.959576	462363.477000	45.911297
3504.671906	462330.092400	45.916301
3504.206398	462370.995114	45.921306
3504.267232	462356.682581	45.926311
3504.836657	462320.987458	45.931316
3504.270716	462307.839066	45.936321
3504.240707	462344.767591	45.941325
3503.931790	462336.346224	45.946330
3504.283677	462303.576466	45.951335
3504.201577	462323.572913	45.956340
3504.003964	462355.253078	45.961345
3504.175600	462333.873011	45.966349
3503.871515	462291.012287	45.971354
3504.183688	462273.008163	45.976359
3504.417569	462269.572945	45.981364
3503.845987	462317.948313	45.986369
3504.174923	462287.160220	45.991373
3504.076165	462299.602097	45.996378
3504.201343	462283.656319	46.001383
3503.713221	462315.940372	46.006388
3504.010401	462285.968810	46.011393
3503.957310	462319.401372	46.016397
3503.820606	462302.939084	46.021402
3503.612099	462302.566247	46.026407
3504.313853	462269.436823	46.031412
3503.966007	462327.565701	46.036417
3503.759858	462328.663357	46.041421
3503.522712	462304.203259	46.046426
3504.360978	462283.072818	46.051431
3504.170566	462269.154974	46.056436
3503.836193	462307.501098	46.061441
3503.964833	462301.445101	46.066445
3504.587729	462273.653704	46.071450
3503.739216	462268.005736	46.076455
3504.213395	462285.175435	46.081460
3503.784434	462293.409056	46.086465
3503.688232	462270.448231	46.091469
3504.468190	462277.121356	46.096474
3504.071973	462263.489635	46.101479
3504.152903	462249.630332	46.106484
3503.803562	462301.825308	46.111489
3503.908813	462289.585214	46.116493
3504.250103	462258.998007	46.121498
3503.786497	462270.533891	46.126503
3504.250833	462317.122503	46.131508
3504.219470	462303.128824	46.136513
3503.847380	462261.141023	46.141517
3503.502430	462253.080357	46.146522
3503.832960	462261.498269	46.151527
3504.483858	462229.746254	46.156532
3503.972380	462255.795557	46.161537
3503.839340	462267.837113	46.166541
3503.835114	462245.521081	46.171546
3504.113755	462222.196643	46.176551
3503.902982	462250.480815	46.181556
3503.927524	462272.235644	46.186561
3503.407029	462248.885380	46.191565
3504.205150	462227.406192	46.196570
3504.017820	462246.658545	46.201575
3504.103170	462263.940435	46.206580
3503.949500	462266.247073	46.211585
3503.702124	462291.341638	46.216589
3504.051031	462263.086335	46.221594
3503.454918	462255.927601	46.226599
3504.029305	462248.025949	46.231604
3504.221004	462246.068266	46.236609
3504.243324	462241.550647	46.241613
3504.590611	462234.039921	46.246618
3504.429214	462236.702821	46.251623
3504.365968	462197.861428	46.256628
3503.983938	462217.601057	46.261633
3503.791599	462236.245574	46.266637
3504.093168	462198.360916	46.271642
3503.950758	462237.843379	46.276647
3503.917707	462225.777267	46.281652
3504.442076	462199.066462	46.286657
3504.231069	462246.624201	46.291661
3504.401635	462212.361373	46.296666
3503.961756	462242.811997	46.301671
3504.281747	462188.998412	46.306676
3503.956070	462202.186287	46.311681
3503.992020	462190.261409	46.316685
3504.179542	462173.189860	46.321690
3503.752756	462207.138137	46.326695
3503.782156	462182.432894	46.331700
3503.904982	462191.492300	46.336705
3503.749920	462192.125410	46.341709
3504.443739	462166.605060	46.346714
3504.214388	462212.948495	46.351719
3504.242625	462206.401142	46.356724
3504.157186	462176.591342	46.361729
3504.071259	462214.999801	46.366733
3503.967850	462190.974916	46.371738
3504.198550	462192.358574	46.376743
3503.804695	462184.609931	46.381748
3504.267096	462141.424888	46.386753
3503.817026	462186.687425	46.391757
3504.097936	462185.780754	46.396762
3503.706347	462187.212046	46.401767
3503.713783	462172.451352	46.406772
3503.971934	462161.252137	46.411777
3504.393575	462151.447235	46.416781
3504.486732	462145.548962	46.421786
3504.137177	462168.428141	46.426791
3503.884214	462167.301528	46.431796
3503.982988	462193.254455	46.436801
3503.983685	462205.731387	46.441805
3504.084012	462206.628451	46.446810
3503.726024	462222.103812	46.451815
3504.012420	462195.227735	46.456820
3503.756598	462183.298248	46.461825
3503.900348	462160.654422	46.466829
3503.959358	462210.908439	46.471834
3503.683926	462192.743520	46.476839
3503.868940	462169.383103	46.481844
3504.152418	462196.118352	46.486849
3503.995510	462186.303466	46.491853
3504.115084	462149.208286	46.496858
3504.136515	462165.587398	46.501863
3504.506923	462126.829498	46.506868
3504.241725	462177.033394	46.511873
3504.035335	462156.422979	46.516877
3504.973533	462118.843322	46.521882
3504.158974	462144.991380	46.526887
3504.082002	462141.453113	46.531892
3504.112691	462138.760069	46.536897
3504.024028	462130.861731	46.541901
3504.206642	462098.524178	46.546906
3504.336715	462082.729640	46.551911
3504.579800	462104.450095	46.556916
3503.947116	462102.876294	46.561921
3504.092648	462066.182630	46.566925
3504.947929	462041.346696	46.571930
3504.113924	462076.779702	46.576935
3504.508564	462098.425490	46.581940
3504.451305	462080.783916	46.586945
3504.198851	462034.110517	46.591949
3504.550427	462033.344832	46.596954
3504.355356	462037.839006	46.601959
3504.554692	462037.553864	46.606964
3504.144792	462027.626731	46.611969
3504.342862	461998.989164	46.616973
3504.653508	462023.032156	46.621978
3504.085807	462008.768015	46.626983
3504.482811	461982.685718	46.631988
3504.686079	462010.499000	46.636993
3504.228474	461976.994447	46.641997
3504.849869	461935.711241	46.647002
3503.998721	461988.290603	46.652007
3504.392584	461955.615128	46.657012
3504.491438	461958.744132	46.662017
3504.002379	461944.518239	46.667021
3504.266286	461915.768716	46.672026
3504.292405	461910.540342	46.677031
3504.204321	461955.999748	46.682036
3504.314783	461925.144233	46.687041
3504.352838	461915.704174	46.692045
3504.262054	461919.218201	46.697050
3504.117294	461887.845046	46.702055
3504.205320	461911.162539	46.707060
3504.677360	461888.060779	46.712065
3504.161059	461883.577495	46.717069
3504.290124	461908.410122	46.722074
3504.279537	461843.387976	46.727079
3504.327143	461869.298656	46.732084
3504.240743	461842.836110	46.737089
3504.361637	461837.795621	46.742093
3504.257656	461872.657091	46.747098
3504.080924	461875.221018	46.752103
3503.907941	461848.772163	46.757108
3503.681984	461833.845245	46.762113
3504.387636	461828.864495	46.767117
3504.075598	461851.027987	46.772122
3503.817157	461831.084858	46.777127
3504.033839	461784.336775	46.782132
3504.083123	461825.362033	46.787137
3504.307348	461840.339880	46.792141
3504.434714	461827.385941	46.797146
3504.319145	461847.641718	46.802151
3504.491052	461834.680744	46.807156
3504.494976	461800.646489	46.812161
3504.145708	461807.954722	46.817165
3504.325453	461781.855803	46.822170
3504.411388	461750.953197	46.827175
3504.695848	461744.669534	46.832180
3504.052006	461739.191960	46.837185
3504.116804	461734.008151	46.842189
3504.477506	461723.198271	46.847194
3504.308158	461709.530344	46.852199
3504.195511	461708.330809	46.857204
3504.190502	461709.903915	46.862209
3503.915240	461752.654397	46.867213
3503.950182	461747.931798	46.872218
3503.890920	461717.559302	46.877223
3503.813272	461707.478068	46.882228
3503.540114	461706.050297	46.887233
3503.937841	461720.493594	46.892237
3504.637793	461707.753412	46.897242
3504.288559	461681.585816	46.902247
3504.187870	461717.765760	46.907252
3504.462445	461733.395095	46.912257
3503.898503	461739.925746	46.917261
3503.738014	461721.032173	46.922266
3503.730478	461683.550522	46.927271
3503.680480	461708.513120	46.932276
3503.865135	461739.930878	46.937281
3503.575622	461734.904510	46.942285
3504.021200	461731.080703	46.947290
3503.796337	461741.615435	46.952295
3503.900722	461696.000771	46.957300
3504.600702	461680.065145	46.962305
3503.708206	461715.203656	46.967309
3504.057931	461719.763953	46.972314
3503.954911	461717.852803	46.977319
3504.093526	461725.692605	46.982324
3503.920323	461719.126223	46.987329
3503.468650	461723.305971	46.992333
3504.208394	461729.732018	46.997338
3503.886551	461761.077635	47.002343
3503.782658	461751.659940	47.007348
3504.087598	461740.199510	47.012353
3503.900416	461703.101332	47.017357
3504.003613	461668.746854	47.022362
3503.759247	461676.038551	47.027367
3504.319041	461707.904275	47.032372
3504.073880	461713.877340	47.037377
3503.914455	461700.309281	47.042381
3504.256218	461686.662000	47.047386
3504.146424	461707.627089	47.052391
3504.103864	461705.554220	47.057396
3503.875737	461678.150175	47.062401
3503.907191	461675.558395	47.067405
3504.034167	461707.340364	47.072410
3503.541840	461704.374882	47.077415
3504.173716	461664.864741	47.082420
3504.223365	461658.668887	47.087425
3503.943504	461697.666843	47.092429
3504.094168	461726.351059	47.097434
3503.981336	461711.558341	47.102439
3503.871933	461668.868504	47.107444
3504.394701	461637.643090	47.112449
3503.783817	461683.134974	47.117453
3503.754701	461660.061460	47.122458
3504.108165	461657.063736	47.127463
3504.166161	461673.538882	47.132468
3503.820076	461661.521932	47.137473
3503.378555	461662.301775	47.142477
3503.995505	461634.054013	47.147482
3504.258581	461628.635956	47.152487
3503.848716	461671.002103	47.157492
3503.769238	461674.412940	47.162497
3503.895802	461652.582839	47.167501
3504.088656	461677.253484	47.172506
3503.973739	461663.729089	47.177511
3504.043849	461663.109319	47.182516
3504.120243	461703.420427	47.187521
3503.718044	461677.413360	47.192525
3504.374315	461661.484629	47.197530
3504.246037	461697.212478	47.202535
3504.126828	461668.117413	47.207540
3504.435857	461630.281310	47.212545
3504.005792	461659.108121	47.217549
3503.860970	461645.486998	47.222554
3504.014789	461629.029004	47.227559
3504.196966	461626.362674	47.232564
3504.172360	461665.827555	47.237569
3503.599986	461664.954284	47.242573
3503.944793	461656.784378	47.247578
3503.968841	461657.845685	47.252583
3503.759771	461646.973657	47.257588
3503.606270	461649.026727	47.262593
3503.531357	461651.828192	47.267597
3503.596449	461638.630378	47.272602
3504.190446	461622.457856	47.277607
3503.874757	461607.900013	47.282612
3504.054467	461610.864125	47.287617
3504.049338	461627.755053	47.292621
3504.125666	461639.155211	47.297626
3504.235140	461671.599373	47.302631
3504.020117	461677.314079	47.307636
3504.040481	461660.623596	47.312641
3503.899222	461637.821388	47.317645
3504.164802	461621.041397	47.322650
3503.901210	461664.398861	47.327655
3504.094312	461684.910330	47.332660
3504.217838	461646.241316	47.337665
3503.895564	461605.715287	47.342669
3504.041893	461635.921944	47.347674
3503.970690	461629.948067	47.352679
3503.814155	461613.894160	47.357684
3504.229637	461588.822896	47.362689
3503.820921	461631.341102	47.367693
3504.078997	461608.272864	47.372698
3503.866230	461640.210070	47.377703
3503.834936	461630.527242	47.382708
3504.378483	461594.936464	47.387713
3504.183756	461653.144383	47.392717
3504.172295	461628.546412	47.397722
3504.391930	461599.397700	47.402727
3504.194508	461580.966334	47.407732
3504.271589	461629.697199	47.412737
3504.103166	461608.319445	47.417741
3503.885241	461582.486024	47.422746
3504.105569	461573.727107	47.427751
3503.756446	461559.377402	47.432756
3504.164861	461569.609240	47.437761
3503.872908	461604.855897	47.442765
3504.030083	461614.214442	47.447770
3503.985615	461600.526709	47.452775
3503.896722	461587.302481	47.457780
3504.196825	461573.712435	47.462785
3504.325527	461621.167128	47.467789
3504.497134	461560.730969	47.472794
3504.397285	461537.617783	47.477799
3504.217337	461569.651348	47.482804
3504.525948	461560.827751	47.487809
3504.256580	461546.719038	47.492813
3504.467931	461567.329177	47.497818
3503.947558	461537.485800	47.502823
3503.919411	461504.115528	47.507828
3504.540274	461485.706915	47.512833
3504.074328	461495.113275	47.517837
3504.342174	461506.432511	47.522842
3504.260746	461515.321596	47.527847
3504.085090	461496.075175	47.532852
3504.477786	461463.906363	47.537857
3504.315704	461443.643320	47.542861
3504.321845	461432.737170	47.547866
3504.422921	461428.714152	47.552871
3504.637494	461437.505763	47.557876
3504.798645	461424.444803	47.562881
3503.607815	461446.189661	47.567885
3503.996252	461431.824743	47.572890
3503.755732	461438.963746	47.577895
3503.776568	461449.307621	47.582900
3503.909906	461442.439098	47.587905
3503.580566	461441.628848	47.592909
3503.985178	461439.333113	47.597914
3503.930282	461450.906274	47.602919
3504.103329	461463.965050	47.607924
3504.007077	461450.539015	47.612929
3504.163308	461434.841316	47.617933
3504.628297	461423.051094	47.622938
3504.555160	461465.415141	47.627943
3504.030879	461424.464208	47.632948
3504.478152	461379.606235	47.637953
3504.225698	461404.195406	47.642957
3504.182869	461417.034721	47.647962
3504.026435	461386.322070	47.652967
3504.068317	461429.733163	47.657972
3504.050391	461416.193284	47.662977
3503.828829	461406.591152	47.667981
3504.001080	461413.918533	47.672986
3504.220566	461403.282979	47.677991
3503.786368	461380.983297	47.682996
3504.028464	461399.154091	47.688001
3503.806312	461382.248117	47.693005
3503.887668	461370.264892	47.698010
3503.959958	461402.918217	47.703015
3504.009058	461378.006062	47.708020
3504.025381	461388.249235	47.713025
3503.925087	461378.425037	47.718029
3504.091224	461405.737742	47.723034
3504.196288	461375.490963	47.728039
3504.100841	461403.098624	47.733044
3504.311549	461383.689595	47.738049
3503.897759	461382.182587	47.743053
3503.880244	461388.829865	47.748058
3503.829126	461395.938947	47.753063
3504.181324	461398.013558	47.758068
3504.179093	461390.963558	47.763073
3503.681595	461409.707734	47.768077
3504.084761	461383.116530	47.773082
3504.063103	461393.517869	47.778087
3503.855103	461353.277640	47.783092
3504.275273	461325.517078	47.788097
3504.054452	461370.288578	47.793101
3504.405826	461369.827234	47.798106
3503.883062	461357.482988	47.803111
3504.236307	461322.023286	47.808116
3504.370988	461364.202517	47.813121
3503.908700	461361.130797	47.818125
3504.775039	461330.256417	47.823130
3504.330094	461347.572127	47.828135
3504.398828	461312.461708	47.833140
3504.106694	461332.847314	47.838145
3503.867137	461307.625648	47.843149
3503.648425	461330.282137	47.848154
3504.075236	461298.767074	47.853159
3504.353692	461304.099551	47.858164
3504.499145	461294.642249	47.863169
3504.226522	461311.322089	47.868173
3504.057578	461305.870791	47.873178
3504.121837	461307.179368	47.878183
3503.809015	461292.062921	47.883188
3503.615225	461287.680705	47.888193
3503.623224	461302.338043	47.893197
3504.111950	461315.752789	47.898202
3503.892699	461307.063241	47.903207
3503.833654	461295.913716	47.908212
3504.327682	461307.603083	47.913217
3503.694931	461292.892254	47.918221
3504.201032	461256.647458	47.923226
3504.227326	461263.135685	47.928231
3503.647421	461278.088846	47.933236
3503.699501	461290.913234	47.938241
3503.788517	461297.594425	47.943245
3503.786035	461281.465204	47.948250
3503.588681	461281.851414	47.953255
3503.972915	461259.980195	47.958260
3504.098974	461301.349359	47.963265
3503.860624	461316.552843	47.968269
3503.540797	461300.068017	47.973274
3503.456507	461303.834725	47.978279
3503.715289	461297.352105	47.983284
3503.980839	461274.941718	47.988289
3503.886677	461296.817727	47.993293
3504.038017	461313.126226	47.998298
3503.842521	461301.237442	48.003303
3503.819367	461277.959694	48.008308
3504.161463	461316.149922	48.013313
3503.860267	461314.320781	48.018317
3504.337693	461274.225683	48.023322
3504.303229	461294.570599	48.028327
3503.994988	461345.036823	48.033332
3503.750671	461319.460871	48.038337
3504.100507	461296.732853	48.043341
3504.254722	461328.866122	48.048346
3504.127125	461313.111752	48.053351
3503.484371	461283.287370	48.058356
3504.336286	461267.327431	48.063361
3504.335253	461250.893626	48.068365
3503.841949	461298.599495	48.073370
3504.128600	461279.533425	48.078375
3504.331423	461258.198096	48.083380
3504.396793	461298.816026	48.088385
3504.095179	461292.574142	48.093389
3504.086663	461278.018252	48.098394
3503.695897	461273.159946	48.103399
3503.621180	461276.925146	48.108404
3504.138991	461267.713312	48.113409
3504.173421	461261.874805	48.118413
3504.368749	461250.634331	48.123418
3504.308040	461267.229990	48.128423
3504.299604	461263.274971	48.133428
3504.644903	461229.135147	48.138433
3504.123483	461236.825834	48.143437
3504.285053	461255.922473	48.148442
3503.985346	461223.456966	48.153447
3504.225451	461182.841266	48.158452
3504.232311	461175.891205	48.163457
3504.310295	461170.908067	48.168461
3503.678024	461195.202448	48.173466
3503.955575	461235.330462	48.178471
3504.018712	461228.878743	48.183476
3503.690910	461197.990024	48.188481
3504.087690	461178.551404	48.193485
3504.257865	461203.530504	48.198490
3504.567756	461223.668893	48.203495
3503.947159	461194.956774	48.208500
3503.564634	461176.351433	48.213505
3504.241523	461172.693860	48.218509
3504.243217	461190.598491	48.223514
3504.149511	461201.062031	48.228519
3503.547037	461175.796128	48.233524
3503.283119	461174.874083	48.238529
3503.813983	461189.398136	48.243533
3504.107582	461192.597915	48.248538
3504.428928	461194.119478	48.253543
3503.928159	461205.205296	48.258548
3503.876646	461197.148581	48.263553
3503.925220	461198.256756	48.268557
3503.589638	461182.940941	48.273562
3503.411441	461176.375184	48.278567
3503.705081	461172.575295	48.283572
3503.917110	461175.128580	48.288577
3503.591563	461184.969382	48.293581
3503.786191	461188.032639	48.298586
3504.717786	461170.538371	48.303591
3504.071076	461185.806487	48.308596
3504.203368	461206.378740	48.313601
3504.129772	461213.491435	48.318605
3504.102674	461184.837665	48.323610
3504.529873	461171.024393	48.328615
3504.477975	461158.504169	48.333620
3504.545237	461172.289949	48.338625
3504.126513	461148.618084	48.343629
3503.829936	461154.295094	48.348634
3504.350725	461131.742776	48.353639
3504.007946	461173.997838	48.358644
3504.326302	461140.318633	48.363649
3504.512655	461133.847413	48.368653
3504.207630	461131.511638	48.373658
3504.387915	461103.332208	48.378663
3504.204949	461122.280529	48.383668
3504.658119	461071.638645	48.388673
3504.016086	461134.686553	48.393677
3504.273400	461086.916109	48.398682
3504.326543	461062.814515	48.403687
3504.017125	461078.485898	48.408692
3504.236375	461059.379567	48.413697
3504.137484	461095.357368	48.418701
3504.120591	461062.593311	48.423706
3504.609683	461081.131113	48.428711
3503.870530	461063.038543	48.433716
3504.510449	461004.403559	48.438721
3504.148638	461055.944092	48.443725
3504.007628	461014.475310	48.448730
3504.845033	460996.539288	48.453735
3504.238816	460997.750964	48.458740
3504.313148	461022.897585	48.463745
3504.174008	461017.695117	48.468749
3504.097353	460980.882576	48.473754
3504.087990	460999.144171	48.478759
3503.941309	460993.384939	48.483764
3504.686814	460957.659760	48.488769
3504.283153	460996.932146	48.493773
3503.995560	460999.716586	48.498778
3504.106980	460975.605685	48.503783
3504.177356	460946.834752	48.508788
3504.401596	460947.915175	48.513793
3503.913256	460985.577838	48.518797
3504.016420	460951.272960	48.523802
3504.375888	460926.564850	48.528807
3504.170688	460947.038519	48.533812
3504.267391	460983.695709	48.538817
3504.099259	460993.410272	48.543821
3504.020705	460975.872614	48.548826
3503.862164	460971.687654	48.553831
3503.868737	460965.802748	48.558836
3503.900185	460941.146498	48.563841
3504.019944	460932.149606	48.568845
3503.555591	460910.767219	48.573850
3503.966185	460935.353566	48.578855
3503.791207	460927.062651	48.583860
3504.109010	460922.599504	48.588865
3503.850192	460943.588879	48.593869
3503.970806	460909.331900	48.598874
3504.536152	460891.793851	48.603879
3503.674270	460924.696985	48.608884
3503.909321	460938.405671	48.613889
3503.826432	460922.390338	48.618893
3504.381478	460893.339842	48.623898
3504.217753	460900.162546	48.628903
3503.766498	460951.007343	48.633908
3504.346759	460905.823043	48.638913
3504.345943	460931.945380	48.643917
3504.102941	460925.186899	48.648922
3504.237038	460887.529328	48.653927
3503.812195	460922.950255	48.658932
3503.969976	460887.875803	48.663937
3504.142738	460891.906292	48.668941
3503.985893	460897.764175	48.673946
3503.767697	460878.016704	48.678951
3503.929001	460868.505990	48.683956
3504.249566	460888.237219	48.688961
3503.980524	460909.583303	48.693965
3503.553667	460902.650982	48.698970
3503.880990	460875.563922	48.703975
3504.145227	460866.493444	48.708980
3504.165399	460904.329490	48.713985
3503.915535	460931.302756	48.718989
3504.017866	460915.917540	48.723994
3503.884666	460897.931952	48.728999
3503.521609	460892.714121	48.734004
3503.822980	460887.289829	48.739009
3503.796516	460886.685302	48.744013
3503.804482	460882.474008	48.749018
3504.100825	460919.353366	48.754023
3503.823048	460906.006410	48.759028
3503.889575	460891.894908	48.764033
3504.074565	460889.380213	48.769037
3504.076656	460926.864018	48.774042
3504.245663	460914.511630	48.779047
3503.940112	460910.451339	48.784052
3504.200242	460876.070812	48.789057
3504.215127	460911.828041	48.794061
3503.839780	460901.894931	48.799066
3503.722983	460888.066015	48.804071
3503.212469	460887.436547	48.809076
3503.509065	460885.462165	48.814081
3504.048260	460884.210282	48.819085
3504.305174	460902.632763	48.824090
3504.173778	460906.508431	48.829095
3504.126956	460871.161953	48.834100
3503.900693	460910.305010	48.839105
3503.747539	460903.633767	48.844109
3503.804246	460898.095979	48.849114
3504.279400	460902.433732	48.854119
3503.916909	460906.447371	48.859124
3504.036732	460907.442853	48.864129
3503.843318	460914.473137	48.869133
3504.170379	460909.856355	48.874138
3504.189448	460878.100794	48.879143
3504.377325	460859.861537	48.884148
3504.197886	460865.266493	48.889153
3504.250174	460908.676976	48.894157
3503.904636	460897.724697	48.899162
3503.956255	460885.390847	48.904167
3504.049486	460872.441737	48.909172
3503.801087	460838.547308	48.914177
3503.811049	460839.509435	48.919181
3503.937229	460813.214933	48.924186
3504.022039	460818.070905	48.929191
3503.928183	460880.474950	48.934196
3503.936962	460872.510032	48.939201
3503.879327	460857.961625	48.944205
3503.517927	460840.772902	48.949210
3504.420814	460832.717376	48.954215
3504.238981	460827.876671	48.959220
3504.377879	460821.412859	48.964225
3504.147591	460835.753110	48.969229
3503.893264	460829.757234	48.974234
3503.797510	460854.677316	48.979239
3503.670401	460879.805218	48.984244
3503.858739	460872.217703	48.989249
3504.044154	460886.086435	48.994253
3503.981782	460888.175896	48.999258
3503.779606	460872.534441	49.004263
3503.448205	460871.065096	49.009268
3503.563292	460855.272039	49.014273
3503.584729	460860.290187	49.019277
3503.606090	460867.945938	49.024282
3504.436616	460830.786872	49.029287
3503.815688	460849.246696	49.034292
3503.603371	460862.214570	49.039297
3503.632090	460865.659155	49.044301
3503.770211	460871.724039	49.049306
3503.571022	460859.125477	49.054311
3504.031293	460853.219556	49.059316
3504.297113	460839.228690	49.064321
3503.893918	460864.552413	49.069325
3503.807803	460880.543705	49.074330
3503.909462	460895.186514	49.079335
3503.820712	460860.303151	49.084340
3503.838002	460851.423866	49.089345
3503.618956	460874.588109	49.094349
3504.285644	460854.852929	49.099354
3504.455966	460856.905615	49.104359
3504.267576	460846.232810	49.109364
3504.346982	460844.140582	49.114369
3503.752688	460850.625570	49.119373
3503.867585	460860.346181	49.124378
3504.485084	460865.320842	49.129383
3503.992345	460875.593991	49.134388
3504.014987	460878.785920	49.139393
3503.911738	460875.961720	49.144397
3503.863882	460878.759008	49.149402
3504.309043	460870.522226	49.154407
3504.062699	460829.729141	49.159412
3504.229465	460834.014203	49.164417
3504.017353	460864.329302	49.169421
3503.691676	460849.772532	49.174426
3504.481373	460822.764496	49.179431
3503.979227	460851.705209	49.184436
3504.075174	460871.218339	49.189441
3504.157254	460843.003372	49.194445
3504.025697	460816.851057	49.199450
3503.931321	460800.583835	49.204455
3503.443980	460810.247485	49.209460
3503.545409	460805.057666	49.214465
3503.948214	460809.914103	49.219469
3504.150303	460802.933068	49.224474
3504.425976	460832.663885	49.229479
3503.650541	460814.678288	49.234484
3503.582128	460806.370484	49.239489
3504.050119	460788.137618	49.244493
3503.988124	460791.545828	49.249498
3504.036590	460818.674974	49.254503
3503.581464	460806.015386	49.259508
3503.935024	460808.546346	49.264513
3503.978715	460834.712488	49.269517
3503.842274	460829.205210	49.274522
3504.074596	460818.668789	49.279527
3504.011132	460818.628061	49.284532
3503.728359	460800.868926	49.289537
3504.066322	460806.851520	49.294541
3504.127161	460833.522184	49.299546
3503.973969	460809.250029	49.304551
3503.507948	460816.881383	49.309556
3504.136939	460783.000364	49.314561
3504.082533	460787.523285	49.319565
3503.866772	460842.287516	49.324570
3503.885491	460829.350157	49.329575
3504.228614	460802.919909	49.334580
3504.009705	460820.200310	49.339585
3503.862151	460844.773530	49.344589
3503.911542	460817.527433	49.349594
3504.379163	460809.946479	49.354599
3504.033221	460814.109687	49.359604
3504.613052	460782.823313	49.364609
3504.239565	460788.360403	49.369613
3503.865341	460809.520316	49.374618
3504.271813	460765.935611	49.379623
3504.304261	460755.532197	49.384628
3504.081545	460761.552697	49.389633
3504.271520	460794.999901	49.394637
3504.074190	460774.538916	49.399642
3504.413542	460726.703997	49.404647
3503.946983	460787.493346	49.409652
3503.984306	460758.981007	49.414657
3504.062468	460732.288212	49.419661
3503.974249	460777.952984	49.424666
3503.976161	460767.148617	49.429671
3504.333591	460744.266657	49.434676
3504.226822	460748.037014	49.439681
3504.232249	460774.158553	49.444685
3504.175952	460753.168025	49.449690
3504.088471	460717.624833	49.454695
3503.888185	460723.083842	49.459700
3503.907051	460720.646109	49.464705
3504.649547	460692.630908	49.469709
3504.480504	460691.744570	49.474714
3504.548629	460734.493493	49.479719
3504.216329	460718.618877	49.484724
3504.131504	460670.850879	49.489729
3504.209742	460664.853118	49.494733
3504.090653	460668.371819	49.499738
3504.296337	460666.665403	49.504743
3503.606986	460677.172612	49.509748
3504.085161	460669.995728	49.514753
3504.895345	460651.049260	49.519757
3504.613147	460629.891425	49.524762
3504.507557	460620.524234	49.529767
3504.583481	460623.707778	49.534772
3504.722999	460602.432540	49.539777
3504.474876	460570.008634	49.544781
3504.430632	460568.595330	49.549786
3504.930741	460560.349748	49.554791
3504.281261	460558.372695	49.559796
3504.191862	460589.429633	49.564801
3504.335772	460573.479647	49.569805
3503.729579	460559.524979	49.574810
3504.443542	460524.920001	49.579815
3504.034283	460541.774193	49.584820
3503.901504	460564.772957	49.589825
3504.145771	460543.075316	49.594829
3503.954477	460572.119437	49.599834
3504.635916	460524.990866	49.604839
3503.854433	460541.396651	49.609844
3504.033120	460494.195303	49.614849
3503.948715	460520.838580	49.619853
3504.136636	460489.918073	49.624858
3503.835172	460526.334616	49.629863
3503.701754	460494.805496	49.634868
3504.001892	460517.735886	49.639873
3503.350483	460492.831992	49.644877
3504.040207	460489.273727	49.649882
3504.156019	460527.247479	49.654887
3503.628040	460507.041398	49.659892
3503.862870	460517.301167	49.664897
3503.752835	460507.731735	49.669901
3503.969831	460494.559946	49.674906
3503.622749	460525.049018	49.679911
3503.857897	460506.446929	49.684916
3504.048639	460529.901834	49.689921
3504.411866	460515.895367	49.694925
3503.741574	460532.841547	49.699930
3504.346516	460491.253875	49.704935
3504.079294	460543.896585	49.709940
3504.142264	460537.698308	49.714945
3503.925757	460516.022744	49.719949
3503.758693	460525.382278	49.724954
3503.847371	460561.584930	49.729959
3503.732911	460532.233983	49.734964
3504.443774	460502.955448	49.739969
3503.951746	460547.467153	49.744973
3503.427462	460527.970638	49.749978
3504.183593	460523.438132	49.754983
3503.902950	460533.982260	49.759988
3504.114382	460540.593610	49.764993
3504.075033	460520.411760	49.769997
3503.725173	460521.684390	49.775002
3503.873483	460495.284562	49.780007
3503.675612	460510.330035	49.785012
3504.276378	460519.213149	49.790017
3504.107919	460499.153133	49.795021
3503.650817	460503.993378	49.800026
3504.229625	460507.046734	49.805031
3503.695566	460496.682011	49.810036
3503.733954	460496.828079	49.815041
3503.674056	460519.764648	49.820045
3504.067859	460480.239275	49.825050
3504.005620	460519.965791	49.830055
3503.763210	460501.591348	49.835060
3503.749836	460500.071713	49.840065
3504.372548	460499.668915	49.845069
3503.714945	460492.975828	49.850074
3504.275292	460504.452250	49.855079
3503.990500	460492.272795	49.860084
3503.899269	460504.663781	49.865089
3504.234682	460515.769958	49.870093
3504.153895	460522.427499	49.875098
3504.212750	460493.454898	49.880103
3503.936379	460501.310005	49.885108
3504.111167	460516.144404	49.890113
3504.154829	460503.253634	49.895117
3503.996529	460487.351350	49.900122
3503.898182	460473.316361	49.905127
3504.496674	460471.142055	49.910132
3504.339954	460460.413333	49.915137
3504.041169	460478.264590	49.920141
3503.665884	460460.671971	49.925146
3504.255408	460475.237953	49.930151
3503.992015	460471.627431	49.935156
3503.952823	460487.155079	49.940161
3504.084859	460457.663625	49.945165
3503.813464	460480.684386	49.950170
3504.395536	460441.585702	49.955175
3503.878187	460461.399026	49.960180
3503.848020	460420.368115	49.965185
3504.055701	460428.248191	49.970189
3503.762157	460428.700342	49.975194
3504.325057	460395.945099	49.980199
3503.945479	460457.381027	49.985204
3503.913187	460433.444415	49.990209
3504.324688	460432.060519	49.995213
3503.570497	460462.614022	50.000218
3504.138013	460424.126294	50.005223
3504.135346	460459.988482	50.010228
3503.741249	460427.384540	50.015233
3503.803593	460442.946896	50.020237
3503.687747	460447.225978	50.025242
3504.407011	460410.895370	50.030247
3503.901142	460461.242694	50.035252
3503.852895	460424.272556	50.040257
3504.168020	460428.280630	50.045261
3504.113932	460437.368727	50.050266
3504.118354	460441.679525	50.055271
3503.572459	460430.961574	50.060276
3504.119448	460452.584919	50.065281
3503.861495	460445.777928	50.070285
3503.788015	460438.840331	50.075290
3503.977000	460436.578573	50.080295
3503.914656	460458.805457	50.085300
3503.840927	460428.281285	50.090305
3504.229267	460408.386802	50.095309
3503.592263	460424.719115	50.100314
3504.003080	460404.821077	50.105319
3503.603553	460415.130432	50.110324
3504.380326	460412.116360	50.115329
3504.075843	460412.113724	50.120333
3503.776490	460411.907382	50.125338
3503.927761	460404.984976	50.130343
3504.152210	460403.224850	50.135348
3503.971441	460427.042927	50.140353
3504.299355	460388.339386	50.145357
3503.888229	460415.592394	50.150362
3503.686340	460417.805398	50.155367
3503.735917	460408.565763	50.160372
3504.125082	460381.113251	50.165377
3504.056282	460416.275826	50.170381
3503.889510	460427.715039	50.175386
3504.441406	460394.606465	50.180391
3504.112992	460423.926074	50.185396
3504.066336	460398.419252	50.190401
3504.252175	460405.339032	50.195405
3504.048660	460387.313414	50.200410
3504.111113	460381.267347	50.205415
3503.785333	460395.876598	50.210420
3504.425730	460357.326511	50.215425
3504.224469	460388.857930	50.220429
3503.739595	460365.144947	50.225434
3504.389273	460343.433757	50.230439
3503.645748	460403.862151	50.235444
3503.675928	460398.784945	50.240449
3504.307491	460372.359315	50.245453
3504.339073	460408.672690	50.250458
3504.206301	460354.723254	50.255463
3504.210412	460362.026839	50.260468
3504.001567	460344.509269	50.265473
3504.457600	460322.321424	50.270477
3504.045359	460330.451687	50.275482
3504.039479	460356.676959	50.280487
3504.067335	460331.158281	50.285492
3504.050066	460367.073654	50.290497
3503.787553	460336.274846	50.295501
3503.768889	460361.690546	50.300506
3503.832658	460355.542815	50.305511
3503.931479	460348.628681	50.310516
3503.581129	460356.952050	50.315521
3503.839697	460354.577838	50.320525
3503.724782	460345.465624	50.325530
3503.971592	460357.752540	50.330535
3503.906868	460347.009222	50.335540
3503.786533	460363.767161	50.340545
3503.832400	460348.796265	50.345549
3503.976229	460332.338875	50.350554
3504.396647	460366.003933	50.355559
3503.899794	460353.502850	50.360564
3504.559451	460340.007385	50.365569
3504.151231	460340.782007	50.370573
3504.381225	460311.071978	50.375578
3503.867163	460329.058829	50.380583
3504.272089	460303.581971	50.385588
3503.939358	460324.938690	50.390593
3503.967135	460331.071889	50.395597
3503.650524	460309.716287	50.400602
3504.132156	460318.111070	50.405607
3503.843571	460328.707276	50.410612
3503.994239	460299.364838	50.415617
3504.267827	460343.603775	50.420621
3503.988126	460328.126356	50.425626
3504.347893	460313.055100	50.430631
3504.304352	460291.656321	50.435636
3504.151620	460269.209568	50.440641
3504.011257	460308.745917	50.445645
3503.667449	460284.452584	50.450650
3504.211186	460270.011636	50.455655
3503.641950	460295.920225	50.460660
3503.609471	460272.896504	50.465665
3504.194603	460248.709932	50.470669
3503.952337	460297.595686	50.475674
3503.761655	460280.937506	50.480679
3504.129180	460279.966346	50.485684
3503.928874	460300.592018	50.490689
3504.286260	460271.470491	50.495693
3504.030619	460293.322299	50.500698
3504.275212	460292.573466	50.505703
3504.183847	460281.834326	50.510708
3504.055708	460259.332953	50.515713
3504.079201	460257.452404	50.520717
3504.095170	460226.609428	50.525722
3504.086026	460267.241048	50.530727
3503.910988	460243.276066	50.535732
3503.938757	460214.105111	50.540737
3503.741246	460212.208764	50.545741
3503.598223	460147.303956	50.550746
3504.094801	460082.602216	50.555751
3503.519827	460055.403130	50.560756
3503.408098	459951.282492	50.565761
3503.342087	459895.190923	50.570765
3503.299480	459803.638500	50.575770
3503.204835	459704.535806	50.580775
3503.137963	459596.145447	50.585780
3503.079559	459480.600834	50.590785
3502.700249	459328.481852	50.595789
3502.198498	459230.709534	50.600794
3501.702189	459069.831540	50.605799
3501.918625	458961.646923	50.610804
3501.512004	458789.744885	50.615809
3501.422060	458648.837037	50.620813
3500.960424	458437.322329	50.625818
3500.792903	458302.968523	50.630823
3500.615367	458088.564773	50.635828
3500.110529	457937.470660	50.640833
3499.765496	457710.102937	50.645837
3499.189594	457556.328768	50.650842
3499.090243	457313.648275	50.655847
3498.673953	457128.037516	50.660852
3498.382451	456907.857027	50.665857
3498.594839	456651.929753	50.670861
3497.435667	456460.596625	50.675866
3497.129327	456216.871558	50.680871
3496.767630	455977.566463	50.685876
3496.179518	455760.972981	50.690881
3495.982036	455514.381958	50.695885
3495.293241	455261.168779	50.700890
3495.142542	455003.605861	50.705895
3494.398599	454767.747674	50.710900
3493.986466	454483.177411	50.715905
3493.683608	454250.592796	50.720909
3493.261666	453968.909700	50.725914
3492.716816	453715.808715	50.730919
3492.287570	453409.257640	50.735924
3491.690837	453147.126845	50.740929
3490.912128	452883.905503	50.745933
3489.903177	452581.747939	50.750938
3490.549919	452262.325997	50.755943
3489.492544	452012.737655	50.760948
3488.700917	451743.263883	50.765953
3488.301172	451412.223044	50.770957
3487.498042	451163.346476	50.775962
3487.449328	450864.160766	50.780967
3486.715983	450551.174962	50.785972
3486.477463	450228.718554	50.790977
3485.966736	449948.573382	50.795981
3485.164071	449606.964225	50.800986
3484.627467	449323.161752	50.805991
3483.712021	449025.713356	50.810996
3483.394527	448667.824691	50.816001
3482.985133	448382.975707	50.821005
3482.198050	448047.431429	50.826010
3481.719499	447745.685371	50.831015
3481.029310	447404.584626	50.836020
3480.170927	447091.978356	50.841025
3479.793010	446745.591123	50.846029
3479.083186	446444.981622	50.851034
3478.697457	446123.050454	50.856039
3477.824211	445781.295475	50.861044
3477.104701	445465.752742	50.866049
3476.563190	445108.759319	50.871053
3476.160107	444798.639624	50.876058
3475.306707	444493.053909	50.881063
3474.612103	444128.456226	50.886068
3474.038073	443812.564201	50.891073
3473.093383	443490.229188	50.896077
3472.729661	443126.173203	50.901082
3471.969127	442839.435349	50.906087
3471.109050	442476.564853	50.911092
3470.127024	442163.558578	50.916097
3470.214735	441817.229816	50.921101
3469.412047	441489.109403	50.926106
3468.377961	441180.616890	50.931111
3467.926363	440824.916848	50.936116
3466.917168	440515.929764	50.941121
3466.511664	440166.685774	50.946125
3465.354381	439831.187125	50.951130
3465.170589	439530.586405	50.956135
3464.481193	439173.351684	50.961140
3463.695909	438851.717396	50.966145
3463.580768	438495.651439	50.971149
3462.436017	438183.458091	50.976154
3461.938005	437859.049276	50.981159
3461.344778	437496.723435	50.986164
3460.409918	437179.229317	50.991169
3460.150382	436841.492178	50.996173
3458.772027	436497.504251	51.001178
3458.822398	436163.644165	51.006183
3457.872966	435826.662603	51.011188
3456.970999	435518.637704	51.016193
3456.559817	435151.603293	51.021197
3455.790223	434849.795106	51.026202
3455.031958	434481.663392	51.031207
3453.873739	434180.568867	51.036212
3453.748058	433815.932986	51.041217
3452.947928	433502.434115	51.046221
3452.171904	433189.613176	51.051226
3451.544847	432832.634567	51.056231
3450.659581	432526.500817	51.061236
3449.877393	432173.879636	51.066241
3449.395797	431871.991008	51.071245
3448.942810	431528.018620	51.076250
3448.257117	431219.577974	51.081255
3447.527381	430868.200477	51.086260
3446.409679	430511.521519	51.091265
3446.079340	430224.419880	51.096269
3445.117347	429913.595112	51.101274
3444.847938	429539.856268	51.106279
3444.068566	429241.666649	51.111284
3442.955079	428891.897925	51.116289
3442.545115	428591.839532	51.121293
3441.494869	428242.712544	51.126298
3441.220144	427904.785105	51.131303
3440.370075	427622.994461	51.136308
3438.963619	427277.873017	51.141313
3439.177314	426926.649668	51.146317
3437.950757	426636.095356	51.151322
3437.313121	426314.840562	51.156327
3436.680561	426005.442021	51.161332
3435.913322	425657.455771	51.166337
3435.406684	425374.723766	51.171341
3434.549464	425034.515726	51.176346
3433.892676	424724.039649	51.181351
3433.460025	424410.527465	51.186356
3432.535281	424095.133693	51.191361
3432.089779	423771.481699	51.196365
3430.893080	423471.109799	51.201370
3430.102262	423153.880616	51.206375
3429.865779	422840.014682	51.211380
3429.056045	422514.906848	51.216385
3428.410252	422213.672136	51.221389
3427.760965	421893.789772	51.226394
3427.052073	421579.145989	51.231399
3426.452597	421263.846297	51.236404
3425.414655	420956.842833	51.241409
3425.109051	420636.815522	51.246413
3424.273934	420314.937625	51.251418
3423.430294	420018.587947	51.256423
3422.524804	419721.432010	51.261428
3422.107939	419418.124127	51.266433
3421.545079	419090.879773	51.271437
3420.667190	418789.111494	51.276442
3420.357486	418487.300997	51.281447
3419.863760	418166.868995	51.286452
3418.579721	417861.039454	51.291457
3418.007059	417553.722271	51.296461
3417.163143	417238.340162	51.301466
3416.352539	416959.458138	51.306471
3416.065168	416640.221362	51.311476
3414.883862	416336.976231	51.316481
3414.333914	416032.459381	51.321485
3413.731734	415736.509862	51.326490
3412.862630	415427.209727	51.331495
3412.489496	415137.747657	51.336500
3411.770057	414832.330357	51.341505
3411.216118	414530.110568	51.346509
3410.392285	414210.855720	51.351514
3409.849229	413941.938880	51.356519
3409.252102	413620.736118	51.361524
3408.324405	413315.208923	51.366529
3407.617268	413010.736319	51.371533
3406.569039	412730.326903	51.376538
3406.077742	412423.349384	51.381543
3405.733198	412117.082402	51.386548
3404.528288	411819.537117	51.391553
3404.097240	411539.120560	51.396557
3403.388761	411235.468590	51.401562
3402.651944	410928.133369	51.406567
3402.269828	410634.080081	51.411572
3401.428529	410340.147348	51.416577
3401.165692	410044.951342	51.421581
3400.422038	409748.634092	51.426586
3399.701324	409426.389361	51.431591
3398.770606	409144.479394	51.436596
3397.719617	408854.529853	51.441601
3397.166521	408549.276193	51.446605
3396.632219	408257.765331	51.451610
3396.001464	407970.638147	51.456615
3395.230504	407670.391327	51.461620
3394.318392	407384.294316	51.466625
3393.965029	407093.989145	51.471629
3393.039737	406814.649248	51.476634
3392.495531	406509.831470	51.481639
3391.848968	406224.647555	51.486644
3391.208150	405927.616457	51.491649
3390.614802	405644.350416	51.496653
3389.578399	405350.070459	51.501658
3389.046965	405054.284593	51.506663
3388.291064	404763.436830	51.511668
3387.647454	404471.933214	51.516673
3386.941258	404188.951504	51.521677
3385.890694	403918.704909	51.526682
3385.863008	403617.590013	51.531687
3385.071193	403330.166134	51.536692
3383.895464	403051.772889	51.541697
3383.309736	402762.074538	51.546701
3382.838924	402479.701309	51.551706
3381.993029	402189.835580	51.556711
3381.717865	401910.908772	51.561716
3381.194306	401640.432527	51.566721
3380.382943	401330.396326	51.571725
3379.576203	401051.164863	51.576730
3378.829316	400763.151738	51.581735
3378.529130	400468.608774	51.586740
3377.661470	400180.279138	51.591745
3376.936057	399901.330014	51.596749
3376.253080	399611.008798	51.601754
3375.397274	399330.575626	51.606759
3375.045179	399048.560584	51.611764
3374.055595	398762.957846	51.616769
3373.498521	398480.334836	51.621773
3372.547660	398191.517945	51.626778
3372.050311	397899.677897	51.631783
3371.326415	397626.683496	51.636788
3370.534613	397348.867358	51.641793
3369.895015	397053.991736	51.646797
3369.269836	396780.110461	51.651802
3368.496298	396516.851794	51.656807
3367.724272	396221.074586	51.661812
3366.781100	395948.406304	51.666817
3366.839137	395666.119940	51.671821
3365.868543	395386.510833	51.676826
3364.901792	395116.839613	51.681831
3364.690591	394841.250076	51.686836
3363.937889	394566.633794	51.691841
3363.418270	394278.376279	51.696845
3362.668733	394007.797544	51.701850
3361.734628	393716.422753	51.706855
3361.237151	393441.248634	51.711860
3360.452679	393173.236834	51.716865
3359.864162	392886.732953	51.721869
3358.988144	392609.425485	51.726874
3358.176634	392350.285245	51.731879
3358.123232	392059.240394	51.736884
3357.055494	391787.118246	51.741889
3356.396781	391503.080489	51.746893
3355.762955	391232.360185	51.751898
3355.088574	390956.329960	51.756903
3354.277537	390691.481755	51.761908
3353.342896	390419.302584	51.766913
3352.910081	390120.546366	51.771917
3352.212667	389884.483709	51.776922
3351.842323	389574.219657	51.781927
3350.796283	389334.190860	51.786932
3349.881828	389033.365746	51.791937
3349.290368	388769.689132	51.796941
3348.632928	388525.372339	51.801946
3348.211270	388234.939302	51.806951
3347.155836	387974.559735	51.811956
3346.846703	387699.438409	51.816961
3346.121443	387425.016543	51.821965
3345.555034	387173.174538	51.826970
3344.961372	386889.573136	51.831975
3344.840930	386617.643432	51.836980
3343.585696	386347.671278	51.841985
3343.019491	386071.612026	51.846989
3342.243582	385795.253272	51.851994
3341.696704	385522.670872	51.856999
3340.859335	385251.912580	51.862004
3339.819773	384980.192471	51.867009
3339.608900	384708.008738	51.872013
3339.014521	384448.853790	51.877018
3338.402287	384168.896671	51.882023
3337.766017	383891.357307	51.887028
3336.684066	383621.566889	51.892033
3336.305208	383341.948209	51.897037
3335.402620	383078.763402	51.902042
3334.816196	382813.263267	51.907047
3334.749656	382532.749966	51.912052
3333.400536	382273.597735	51.917057
3333.111778	381994.768776	51.922061
3332.181490	381737.072682	51.927066
3331.620907	381443.785656	51.932071
3330.790245	381169.919665	51.937076
3329.822917	380912.961502	51.942081
3329.101545	380651.104823	51.947085
3328.810235	380382.463716	51.952090
3328.420200	380106.612976	51.957095
3327.552565	379827.096915	51.962100
3326.256603	379575.065355	51.967105
3326.203491	379303.199818	51.972109
3325.516134	379036.443431	51.977114
3324.615234	378763.919750	51.982119
3323.742540	378504.082061	51.987124
3323.284019	378244.507840	51.992129
3322.832789	377973.891609	51.997133
3321.985731	377709.237297	52.002138
3321.436186	377454.734103	52.007143
3320.815410	377174.041103	52.012148
3319.513872	376911.691797	52.017153
3318.793129	376633.885168	52.022157
3318.050683	376388.969945	52.027162
3317.427963	376140.218754	52.032167
3316.766281	375868.655048	52.037172
3315.877621	375606.664434	52.042177
3315.685320	375352.422212	52.047181
3314.920985	375103.559907	52.052186
3314.341492	374845.382058	52.057191
3314.001653	374577.320189	52.062196
3312.691032	374325.079999	52.067201
3312.465632	374065.594808	52.072205
3311.787803	373806.586556	52.077210
3310.849905	373552.527473	52.082215
3310.583166	373291.466797	52.087220
3309.778809	373030.896533	52.092225
3309.458299	372765.058560	52.097229
3308.443708	372511.386875	52.102234
3307.669441	372243.658545	52.107239
3307.082357	371970.607486	52.112244
3306.500831	371725.028702	52.117249
3306.101343	371454.844788	52.122253
3305.315878	371197.185823	52.127258
3304.294890	370947.601651	52.132263
3303.740625	370672.705396	52.137268
3303.176788	370410.427390	52.142273
3302.334725	370149.158532	52.147277
3301.587840	369891.638284	52.152282
3301.136836	369641.625679	52.157287
3300.495957	369384.670801	52.162292
3299.764406	369123.454616	52.167297
3298.969059	368870.769830	52.172301
3298.578479	368602.881848	52.177306
3297.725220	368349.821598	52.182311
3297.296414	368085.091283	52.187316
3296.412519	367829.361498	52.192321
3295.910250	367567.667304	52.197325
3295.048321	367312.668890	52.202330
3294.017415	367042.379384	52.207335
3293.782485	366784.836322	52.212340
3293.064292	366521.083847	52.217345
3292.459135	366263.596346	52.222349
3291.815454	366016.010809	52.227354
3290.759100	365768.590953	52.232359
3290.503110	365481.911335	52.237364
3289.745746	365231.591614	52.242369
3289.535591	364978.079858	52.247373
3288.480472	364719.382582	52.252378
3287.372307	364451.685093	52.257383
3287.024620	364201.981942	52.262388
3285.973692	363959.004147	52.267393
3285.126814	363699.581218	52.272397
3284.324685	363449.793213	52.277402
3284.162154	363198.426929	52.282407
3283.405306	362936.695495	52.287412
3282.397213	362696.223362	52.292417
3282.066732	362442.513208	52.297421
3281.618538	362193.425875	52.302426
3280.813181	361946.683789	52.307431
3280.553918	361688.937971	52.312436
3279.591189	361427.612405	52.317441
3279.077706	361167.944663	52.322445
3278.580869	360912.013414	52.327450
3277.542964	360652.578490	52.332455
3277.251590	360400.072670	52.337460
3276.180269	360151.633045	52.342465
3275.721912	359890.295680	52.347469
3274.836851	359637.243614	52.352474
3274.038302	359385.932367	52.357479
3273.509835	359123.838576	52.362484
3272.639991	358881.747742	52.367489
3271.787827	358626.725831	52.372493
3271.352597	358381.993651	52.377498
3270.619218	358128.909811	52.382503
3270.216233	357881.905251	52.387508
3269.340629	357631.589690	52.392513
3268.936232	357387.992872	52.397517
3268.178046	357130.352750	52.402522
3267.313123	356885.910207	52.407527
3267.038745	356622.185253	52.412532
3266.224409	356374.118605	52.417537
3265.708021	356124.629411	52.422541
3264.839079	355866.796771	52.427546
3264.200996	355619.818295	52.432551
3263.936423	355367.689818	52.437556
3262.900824	355113.162615	52.442561
3262.274238	354863.888289	52.447565
3261.684041	354599.133983	52.452570
3260.708047	354352.508257	52.457575
3260.091074	354088.060968	52.462580
3259.479915	353843.131128	52.467585
3258.754977	353588.089218	52.472589
3258.237668	353344.465580	52.477594
3257.359119	353092.474070	52.482599
3257.116437	352836.792351	52.487604
3256.044735	352589.868078	52.492609
3255.470366	352332.658489	52.497613
3254.884906	352097.922000	52.502618
3254.387920	351850.598002	52.507623
3253.672305	351580.860101	52.512628
3252.889719	351340.857774	52.517633
3252.005457	351081.858763	52.522637
3251.549050	350829.713476	52.527642
3250.727953	350582.638545	52.532647
3250.220699	350327.623018	52.537652
3249.452515	350085.347728	52.542657
3248.928295	349834.023015	52.547661
3248.330873	349575.938652	52.552666
3247.656457	349330.056559	52.557671
3247.020542	349070.525193	52.562676
3246.354842	348824.664939	52.567681
3245.584794	348560.087510	52.572685
3244.944344	348311.853984	52.577690
3244.057040	348063.862026	52.582695
3243.949196	347819.156293	52.587700
3242.797632	347565.069956	52.592705
3242.046401	347314.813391	52.597709
3241.735068	347061.915441	52.602714
3240.613372	346807.286503	52.607719
3240.237447	346552.843913	52.612724
3239.533714	346312.451151	52.617729
3238.898935	346065.123265	52.622733
3238.263840	345809.471204	52.627738
3237.490256	345556.639784	52.632743
3237.179376	345306.228513	52.637748
3235.888886	345068.316047	52.642753
3235.655642	344798.443897	52.647757
3234.960099	344556.388147	52.652762
3234.045194	344304.413681	52.657767
3233.545427	344058.328695	52.662772
3232.711288	343802.292168	52.667777
3232.312715	343563.341715	52.672781
3231.338470	343316.997838	52.677786
3230.891960	343067.005881	52.682791
3230.403485	342806.354135	52.687796
3229.398150	342575.055720	52.692801
3228.701940	342313.314729	52.697805
3228.264740	342064.335379	52.702810
3227.324851	341830.172877	52.707815
3227.176336	341575.418559	52.712820
3226.469077	341325.409845	52.717825
3225.619960	341075.168016	52.722829
3225.104694	340818.661303	52.727834
3224.015586	340561.480651	52.732839
3223.758367	340310.378491	52.737844
3222.882164	340073.526520	52.742849
3222.189260	339818.800277	52.747853
3221.734283	339566.606412	52.752858
3220.909995	339318.441081	52.757863
3220.374320	339069.618196	52.762868
3219.782016	338821.668816	52.767873
3218.745444	338573.050533	52.772877
3218.196372	338329.445431	52.777882
3217.585153	338080.605251	52.782887
3217.170077	337812.029836	52.787892
3216.235682	337566.548164	52.792897
3215.559816	337328.228906	52.797901
3215.250072	337073.711331	52.802906
3214.014205	336830.183876	52.807911
3213.730655	336574.361960	52.812916
3212.847389	336326.321944	52.817921
3212.413157	336077.369904	52.822925
3211.623922	335828.422190	52.827930
3210.690702	335581.863867	52.832935
3210.522250	335337.882161	52.837940
3209.535071	335081.249457	52.842945
3208.974991	334838.677174	52.847949
3208.359057	334578.827143	52.852954
3207.417876	334339.342856	52.857959
3206.984708	334081.269556	52.862964
3206.445527	333849.204598	52.867969
3205.595528	333584.194486	52.872973
3204.916121	333341.915925	52.877978
3204.082176	333084.055124	52.882983
3203.854829	332838.750192	52.887988
3202.782679	332597.727768	52.892993
3202.216044	332343.131600	52.897997
3201.732471	332097.304586	52.903002
3200.929636	331845.188049	52.908007
3200.365648	331597.920928	52.913012
3199.541015	331356.829769	52.918017
3198.858643	331095.831939	52.923021
3198.240743	330852.898850	52.928026
3197.314689	330620.197327	52.933031
3196.745583	330365.620147	52.938036
3195.945519	330125.717681	52.943041
3195.305550	329882.912225	52.948045
3194.838039	329633.561108	52.953050
3194.003367	329386.991416	52.958055
3193.548449	329153.166998	52.963060
3192.987010	328902.733590	52.968065
3192.465290	328660.058292	52.973069
3191.913013	328413.364421	52.978074
3190.493312	328169.505731	52.983079
3190.646303	327917.861350	52.988084
3189.586905	327678.476000	52.993089
3188.964199	327427.818400	52.998093
3188.227407	327179.571311	53.003098
3187.709368	326930.728715	53.008103
3187.103938	326685.361775	53.013108
3186.432114	326428.012735	53.018113
3185.722514	326181.362257	53.023117
3185.140467	325937.695198	53.028122
3183.957300	325693.460527	53.033127
3183.661675	325438.493064	53.038132
3182.878883	325189.559706	53.043137
3182.224095	324955.499960	53.048141
3182.021074	324696.085368	53.053146
3180.997131	324453.425888	53.058151
3180.602550	324206.897902	53.063156
3179.726481	323959.706992	53.068161
3179.088081	323714.056360	53.073165
3178.269972	323463.341187	53.078170
3177.435928	323219.171379	53.083175
3176.956387	322961.144683	53.088180
3176.357156	322718.438541	53.093185
3175.266868	322494.625535	53.098189
3175.119694	322244.335386	53.103194
3174.272050	321993.136869	53.108199
3173.765323	321742.367482	53.113204
3172.949387	321491.569918	53.118209
3172.180191	321252.349450	53.123213
3171.931845	320994.993367	53.128218
3171.136253	320747.984354	53.133223
3170.521726	320500.207623	53.138228
3169.785612	320246.109358	53.143233
3169.058873	320014.288428	53.148237
3168.286896	319757.317249	53.153242
3167.212527	319515.797978	53.158247
3166.630952	319272.214046	53.163252
3166.299499	319030.754232	53.168257
3165.367894	318791.171132	53.173261
3164.991401	318558.221761	53.178266
3164.177934	318311.336433	53.183271
3163.893186	318065.156173	53.188276
3163.072460	317817.965177	53.193281
3162.322082	317561.035571	53.198285
3161.833342	317320.844034	53.203290
3161.010933	317080.628310	53.208295
3160.562153	316817.003182	53.213300
3160.063783	316586.385534	53.218305
3159.246430	316334.759691	53.223309
3158.665420	316083.477780	53.228314
3157.864513	315840.276470	53.233319
3157.293288	315581.098116	53.238324
3156.362504	315347.312203	53.243329
3155.684601	315094.464456	53.248333
3154.797613	314852.191123	53.253338
3154.180375	314606.793445	53.258343
3153.468207	314361.868561	53.263348
3152.720129	314111.626854	53.268353
3152.341126	313868.099562	53.273357
3151.833189	313650.157909	53.278362
3151.026365	313396.511662	53.283367
3150.522447	313132.249319	53.288372
3150.050828	312893.878231	53.293377
3149.303162	312655.626694	53.298381
3148.716334	312403.191092	53.303386
3147.902504	312157.055046	53.308391
3147.190533	311898.068321	53.313396
3146.431803	311661.522532	53.318401
3145.812381	311408.198607	53.323405
3145.124716	311157.049404	53.328410
3144.002022	310917.427531	53.333415
3143.614384	310677.612477	53.338420
3143.151321	310437.019461	53.343425
3142.023272	310189.197327	53.348429
3141.687301	309949.703661	53.353434
3140.746452	309709.999638	53.358439
3140.305514	309461.685317	53.363444
3139.546932	309223.734034	53.368449
3138.937004	308974.325000	53.373453
3138.572092	308741.607212	53.378458
3137.449073	308493.780824	53.383463
3137.329083	308244.572924	53.388468
3136.507408	308005.432429	53.393473
3135.633074	307757.437921	53.398477
3134.860144	307516.760884	53.403482
3134.134270	307275.210132	53.408487
3133.608871	307041.750662	53.413492
3132.793425	306797.615731	53.418497
3131.786650	306557.330438	53.423501
3131.653372	306323.247415	53.428506
3131.197704	306081.600796	53.433511
3130.256318	305836.567274	53.438516
3129.582709	305603.892706	53.443521
3128.691122	305358.239273	53.448525
3128.503214	305119.553538	53.453530
3127.167831	304875.548343	53.458535
3127.072987	304629.767566	53.463540
3126.406160	304400.680597	53.468545
3125.741634	304154.912739	53.473549
3125.592636	303906.949223	53.478554
3124.534372	303673.746619	53.483559
3123.942375	303430.003339	53.488564
3123.480762	303177.937093	53.493569
3122.807673	302934.485958	53.498573
3122.149392	302689.351322	53.503578
3121.239100	302441.964207	53.508583
3121.015882	302185.147345	53.513588
3120.408045	301950.979492	53.518593
3119.275233	301697.539960	53.523597
3118.932166	301435.622103	53.528602
3118.203680	301183.747623	53.533607
3117.741548	300941.940778	53.538612
3116.836137	300697.275067	53.543617
3116.293291	300425.022335	53.548621
3115.837948	300178.603855	53.553626
3114.821478	299931.255134	53.558631
3114.219852	299675.792962	53.563636
3113.306133	299424.276189	53.568641
3112.576316	299171.965952	53.573645
3111.870227	298930.856957	53.578650
3111.231413	298689.023920	53.583655
3110.550944	298443.682728	53.588660
3109.750854	298200.448411	53.593665
3109.018443	297953.994237	53.598669
3108.509905	297700.857449	53.603674
3107.647253	297478.896941	53.608679
3107.258044	297225.995302	53.613684
3106.694804	296992.272046	53.618689
3105.986369	296747.238654	53.623693
3105.484220	296498.275854	53.628698
3104.628733	296252.297364	53.633703
3103.946667	296001.274109	53.638708
3103.022061	295755.076745	53.643713
3102.748674	295512.137711	53.648717
3102.026449	295270.440904	53.653722
3101.000377	295017.102433	53.658727
3100.607925	294774.818068	53.663732
3100.171444	294537.022642	53.668737
3099.409883	294296.502457	53.673741
3098.574924	294050.925620	53.678746
3097.867485	293805.099131	53.683751
3097.112508	293553.371457	53.688756
3096.162293	293322.812377	53.693761
3095.658256	293078.048026	53.698765
3095.181347	292822.353576	53.703770
3094.232891	292601.725837	53.708775
3094.027783	292351.539800	53.713780
3093.534834	292098.164675	53.718785
3092.481138	291866.067060	53.723789
3091.586794	291628.850496	53.728794
3091.492970	291388.552798	53.733799
3090.961739	291129.096009	53.738804
3090.206616	290897.154028	53.743809
3089.343641	290643.861509	53.748813
3088.926169	290398.087647	53.753818
3088.232715	290151.287594	53.758823
3087.590392	289908.095661	53.763828
3086.995781	289658.605428	53.768833
3085.797392	289409.541607	53.773837
3085.260457	289155.635895	53.778842
3084.577952	288919.937059	53.783847
3084.176321	288667.792286	53.788852
3083.391980	288424.265087	53.793857
3082.711780	288186.349635	53.798861
3082.273666	287931.052041	53.803866
3081.279629	287687.914033	53.808871
3080.597660	287445.159427	53.813876
3079.941571	287201.534648	53.818881
3079.230734	286963.572263	53.823885
3078.756851	286725.419420	53.828890
3078.005472	286477.887164	53.833895
3077.400829	286236.774945	53.838900
3076.648769	286006.000474	53.843905
3076.064420	285759.918482	53.848909
3075.384173	285506.440300	53.853914
3074.440616	285269.863525	53.858919
3074.119591	285015.054802	53.863924
3073.506576	284770.326586	53.868929
3072.652944	284518.174146	53.873933
3072.193838	284280.934423	53.878938
3071.801804	284042.614306	53.883943
3071.123540	283797.488425	53.888948
3069.970061	283552.284818	53.893953
3069.263582	283304.056049	53.898957
3069.070809	283062.316679	53.903962
3068.156073	282816.718407	53.908967
3067.678392	282564.301783	53.913972
3067.267081	282324.430404	53.918977
3066.157926	282073.081302	53.923981
3065.720023	281835.811712	53.928986
3064.431042	281594.932881	53.933991
3063.972726	281338.335921	53.938996
3063.614352	281096.825761	53.944001
3063.017710	280854.410903	53.949005
3062.405002	280601.785720	53.954010
3061.430100	280356.960150	53.959015
3060.440343	280112.034991	53.964020
3060.109037	279869.119442	53.969025
3059.073954	279637.597685	53.974029
3059.072999	279386.123318	53.979034
3058.318068	279158.020822	53.984039
3057.510028	278891.647741	53.989044
3056.863244	278666.202221	53.994049
3055.811407	278413.620547	53.999053
3055.712208	278155.819869	54.004058
3054.977236	277920.761153	54.009063
3054.173652	277680.976149	54.014068
3053.432027	277437.794018	54.019073
3052.922060	277181.637264	54.024077
3052.284307	276945.697141	54.029082
3051.272496	276707.931539	54.034087
3051.046331	276455.295395	54.039092
3050.182495	276200.671747	54.044097
3049.090781	275972.800499	54.049101
3048.654155	275722.413394	54.054106
3048.134795	275484.926389	54.059111
3047.532416	275249.464530	54.064116
3046.578220	275010.543718	54.069121
3045.990925	274775.486985	54.074125
3045.588862	274531.181397	54.079130
3044.493177	274283.012529	54.084135
3044.142865	274043.232164	54.089140
3043.327907	273797.565756	54.094145
3042.733611	273566.865331	54.099149
3042.518450	273312.674032	54.104154
3041.318021	273083.164737	54.109159
3040.636764	272827.188089	54.114164
3039.801509	272593.469738	54.119169
3039.344773	272362.314768	54.124173
3038.697033	272108.344961	54.129178
3038.258479	271892.366345	54.134183
3037.627103	271638.113908	54.139188
3036.862857	271399.239969	54.144193
3035.932219	271163.092068	54.149197
3035.275850	270925.372726	54.154202
3034.621715	270686.787175	54.159207
3034.096555	270444.386507	54.164212
3033.684342	270213.657988	54.169217
3032.758412	269956.600232	54.174221
3032.173309	269715.839264	54.179226
3031.442330	269481.901496	54.184231
3030.899907	269248.723488	54.189236
3030.455011	269004.094890	54.194241
3029.300907	268763.016844	54.199245
3029.059218	268512.651405	54.204250
3028.108535	268278.086705	54.209255
3027.466778	268049.712925	54.214260
3027.051768	267799.400714	54.219265
3026.490719	267552.397132	54.224269
3025.884251	267307.005358	54.229274
3024.810799	267067.545291	54.234279
3024.391066	266829.433570	54.239284
3023.848483	266583.369893	54.244289
3023.088185	266335.532574	54.249293
3022.387830	266092.983275	54.254298
3021.806157	265844.608610	54.259303
3021.214005	265598.298667	54.264308
3020.639628	265358.353076	54.269313
3019.778407	265103.299549	54.274317
3019.413742	264866.580981	54.279322
3018.511711	264619.989622	54.284327
3018.121181	264366.568460	54.289332
3017.558987	264110.704254	54.294337
3016.682069	263878.218687	54.299341
3015.945894	263620.294008	54.304346
3015.273103	263379.397529	54.309351
3014.648648	263133.731080	54.314356
3014.031246	262876.755967	54.319361
3012.936427	262610.815537	54.324365
3012.595506	262368.313758	54.329370
3011.453633	262129.096948	54.334375
3010.894962	261876.748519	54.339380
3010.279073	261621.913522	54.344385
3009.677163	261389.870168	54.349389
3009.168272	261133.083124	54.354394
3008.277485	260899.736107	54.359399
3007.899744	260654.643893	54.364404
3007.069473	260404.988411	54.369409
3006.333090	260168.841616	54.374413
3005.839179	259917.019548	54.379418
3004.700016	259677.575226	54.384423
3004.113816	259428.060330	54.389428
3003.587115	259189.512772	54.394433
3002.781158	258957.707600	54.399437
3002.289533	258713.755844	54.404442
3001.743017	258476.358161	54.409447
3001.031902	258242.806884	54.414452
3000.565152	257995.719441	54.419457
3000.154913	257755.957923	54.424461
2999.555031	257491.421479	54.429466
2998.767090	257249.326353	54.434471
2997.825637	257010.617473	54.439476
2997.389327	256754.485698	54.444481
2996.515597	256516.174123	54.449485
2995.933954	256274.276645	54.454490
2995.259223	256031.502828	54.459495
2994.663520	255773.869445	54.464500
2994.056938	255535.236574	54.469505
2993.260978	255293.425108	54.474509
2992.548895	255039.452877	54.479514
2991.805928	254802.141291	54.484519
2991.093009	254553.848969	54.489524
2990.696484	254314.725925	54.494529
2989.868662	254071.622207	54.499533
2989.302165	253825.676084	54.504538
2988.650175	253581.169962	54.509543
2988.140949	253322.558419	54.514548
2987.237839	253083.669943	54.519553
2986.483648	252837.678458	54.524557
2986.277583	252582.534405	54.529562
2985.519610	252350.449022	54.534567
2984.570844	252099.141365	54.539572
2984.071096	251852.576192	54.544577
2983.497514	251605.488264	54.549581
2982.871119	251358.052526	54.554586
2981.959304	251104.168376	54.559591
2981.093115	250850.863123	54.564596
2980.512703	250612.894742	54.569601
2979.881739	250383.083952	54.574605
2979.165996	250133.550497	54.579610
2978.526433	249900.456605	54.584615
2977.686282	249645.417425	54.589620
2977.477682	249409.225562	54.594625
2976.549631	249159.294337	54.599629
2976.093714	248915.451593	54.604634
2975.417278	248668.562747	54.609639
2974.621043	248432.414479	54.614644
2973.900665	248184.311016	54.619649
2973.129596	247936.419721	54.624653
2972.775926	247690.882040	54.629658
2971.818755	247457.511131	54.634663
2971.226001	247222.631364	54.639668
2970.796077	246965.188974	54.644673
2970.029100	246725.575501	54.649677
2969.398995	246481.382409	54.654682
2968.636305	246247.218739	54.659687
2967.886766	245991.254811	54.664692
2967.377697	245754.556204	54.669697
2966.819835	245506.406242	54.674701
2966.216833	245256.965143	54.679706
2965.723168	245020.800161	54.684711
2964.775296	244777.831840	54.689716
2964.157347	244518.412063	54.694721
2963.707925	244268.592005	54.699725
2963.231456	244022.087192	54.704730
2961.895673	243774.878523	54.709735
2961.483784	243532.871769	54.714740
2961.064976	243288.167273	54.719745
2960.184042	243041.779316	54.724749
2959.657425	242787.161497	54.729754
2959.057217	242548.624231	54.734759
2958.089858	242296.980195	54.739764
2957.575081	242050.179752	54.744769
2956.856348	241803.539422	54.749773
2955.984790	241554.300922	54.754778
2955.426758	241315.301046	54.759783
2954.887557	241069.117644	54.764788
2954.348024	240821.559724	54.769793
2953.507530	240572.369310	54.774797
2952.904897	240327.521669	54.779802
2952.312269	240080.075595	54.784807
2951.466275	239832.339126	54.789812
2951.031938	239588.637787	54.794817
2950.123956	239331.261257	54.799821
2949.422772	239085.107756	54.804826
2948.768432	238849.591392	54.809831
2948.368015	238595.319236	54.814836
2947.577875	238350.887545	54.819841
2946.712076	238114.387672	54.824845
2946.431387	237864.528997	54.829850
2945.701729	237615.735063	54.834855
2944.909687	237374.845358	54.839860
2944.305988	237119.768550	54.844865
2943.799599	236878.580117	54.849869
2943.224842	236625.486092	54.854874
2942.514866	236370.758956	54.859879
2941.474210	236125.582674	54.864884
2941.280596	235875.638544	54.869889
2940.706668	235629.472881	54.874893
2940.314590	235369.528844	54.879898
2939.264866	235128.710619	54.884903
2938.498683	234874.454458	54.889908
2938.136471	234615.093299	54.894913
2937.231468	234362.795618	54.899917
2936.449105	234101.694442	54.904922
2935.564789	233853.850814	54.909927
2935.199098	233601.036851	54.914932
2934.724185	233348.011673	54.919937
2933.743032	233115.106455	54.924941
2933.025807	232852.012248	54.929946
2932.608291	232593.632825	54.934951
2932.002353	232346.461976	54.939956
2931.139666	232100.427307	54.944961
2930.492672	231842.671913	54.949965
2930.161947	231575.828050	54.954970
2929.154254	231341.149071	54.959975
2928.337192	231098.827327	54.964980
2928.104724	230833.752416	54.969985
2927.305008	230590.894574	54.974989
2926.490780	230341.164954	54.979994
2925.735457	230088.804131	54.984999
2925.069508	229839.739907	54.990004
2924.332057	229592.953795	54.995009
2923.671548	229340.681934	55.000013
2922.866631	229095.715674	55.005018
2922.337037	228855.977050	55.010023
2921.844046	228602.204031	55.015028
2921.446027	228351.395703	55.020033
2920.515266	228107.597919	55.025037
2919.908384	227850.051414	55.030042
2919.182493	227595.223411	55.035047
2918.610284	227353.560682	55.040052
2918.029907	227097.921849	55.045057
2917.089844	226852.576029	55.050061
2916.767024	226593.295243	55.055066
2915.800364	226357.515643	55.060071
2915.109094	226109.268297	55.065076
2914.600136	225855.900715	55.070081
2913.902286	225622.028408	55.075085
2913.326013	225375.903769	55.080090
2912.490499	225123.455823	55.085095
2911.920834	224874.862007	55.090100
2911.561120	224616.917279	55.095105
2910.601184	224374.790052	55.100109
2910.171262	224117.176311	55.105114
2909.358367	223873.168753	55.110119
2908.546444	223623.306021	55.115124
2908.320325	223362.518187	55.120129
2907.261589	223117.648084	55.125133
2906.598582	222865.574670	55.130138
2906.055926	222621.922875	55.135143
2905.279063	222367.297701	55.140148
2904.724889	222116.635247	55.145153
2903.938019	221872.795370	55.150157
2903.341778	221612.466697	55.155162
2902.717557	221374.458305	55.160167
2902.016343	221130.123547	55.165172
2901.619674	220861.097070	55.170177
2900.817768	220605.565292	55.175181
2900.252989	220354.070264	55.180186
2899.347756	220114.557410	55.185191
2899.028731	219853.401789	55.190196
2898.354718	219596.758551	55.195201
2897.534035	219347.127787	55.200205
2897.087058	219089.101103	55.205210
2896.595291	218836.823277	55.210215
2895.389129	218587.739885	55.215220
2895.065233	218318.303949	55.220225
2894.112034	218066.203736	55.225229
2893.390289	217814.169609	55.230234
2892.991831	217565.483820	55.235239
2892.406970	217305.588837	55.240244
2891.960409	217048.855129	55.245249
2891.113723	216801.057673	55.250253
2890.445218	216533.643387	55.255258
2889.955734	216282.354484	55.260263
2888.742819	216021.660025	55.265268
2888.422837	215760.137844	55.270273
2887.617545	215511.154739	55.275277
2887.051549	215259.118011	55.280282
2886.428557	215000.587018	55.285287
2885.712347	214744.019223	55.290292
2885.125519	214487.801050	55.295297
2883.927862	214242.970567	55.300301
2883.207306	213979.838607	55.305306
2882.987547	213740.913798	55.310311
2882.023393	213486.133890	55.315316
2881.665680	213232.888153	55.320321
2881.014575	212980.618998	55.325325
2880.550103	212730.408665	55.330330
2879.880092	212474.173338	55.335335
2879.158192	212206.224854	55.340340
2878.483808	211953.492466	55.345345
2877.934045	211708.314383	55.350349
2877.248181	211439.739744	55.355354
2876.750264	211175.616631	55.360359
2875.722048	210923.262555	55.365364
2875.015287	210668.809455	55.370369
2874.289804	210408.225681	55.375373
2873.976317	210151.383279	55.380378
2872.980242	209899.931897	55.385383
2872.416058	209649.049522	55.390388
2871.900795	209393.056765	55.395393
2870.836217	209136.273867	55.400397
2870.417472	208888.375206	55.405402
2869.803493	208626.394036	55.410407
2869.038812	208373.194110	55.415412
2868.570750	208116.601062	55.420417
2867.872546	207854.280213	55.425421
2867.262253	207595.522862	55.430426
2866.653282	207347.940634	55.435431
2865.707067	207091.936755	55.440436
2865.189990	206830.597144	55.445441
2864.504887	206576.692247	55.450445
2863.923424	206315.059669	55.455450
2863.495150	206056.560203	55.460455
2862.448668	205798.210669	55.465460
2862.080927	205543.980011	55.470465
2860.795281	205287.337788	55.475469
2860.636146	205035.074383	55.480474
2859.812522	204775.319672	55.485479
2859.221604	204531.195340	55.490484
2859.181016	204262.410570	55.495489
2858.095127	204001.110121	55.500493
2857.177748	203743.563847	55.505498
2856.818786	203484.848610	55.510503
2856.001436	203225.672648	55.515508
2855.418496	202968.242396	55.520513
2854.718054	202711.340966	55.525517
2854.154342	202449.252389	55.530522
2853.205537	202191.705487	55.535527
2852.375058	201939.294954	55.540532
2852.404433	201668.017288	55.545537
2851.393387	201411.972777	55.550541
2850.308240	201159.707949	55.555546
2849.810390	200892.577038	55.560551
2849.382327	200650.174551	55.565556
2848.993049	200389.149836	55.570561
2848.075889	200125.753990	55.575565
2847.513622	199868.436788	55.580570
2846.908781	199606.012049	55.585575
2845.977305	199350.537314	55.590580
2845.585985	199078.206688	55.595585
2844.647755	198829.848809	55.600589
2843.978770	198567.426618	55.605594
2843.545110	198309.714833	55.610599
2842.646304	198053.706734	55.615604
2842.015429	197783.736623	55.620609
2841.123732	197536.420906	55.625613
2840.706353	197276.014002	55.630618
2839.745169	197024.245393	55.635623
2839.362853	196763.402875	55.640628
2838.915038	196506.478438	55.645633
2838.090985	196255.175394	55.650637
2837.199255	195991.656273	55.655642
2836.826514	195735.767198	55.660647
2836.064458	195475.220399	55.665652
2835.591037	195210.710217	55.670657
2834.802589	194963.199683	55.675661
2833.859428	194701.769415	55.680666
2833.331983	194439.485797	55.685671
2832.382042	194191.482956	55.690676
2832.267112	193933.819029	55.695681
2831.555138	193685.870085	55.700685
2830.872003	193419.315875	55.705690
2830.445005	193161.018297	55.710695
2829.483351	192907.603490	55.715700
2828.779108	192642.952616	55.720705
2827.918526	192383.162800	55.725709
2827.409227	192122.911593	55.730714
2826.890852	191872.027501	55.735719
2826.050772	191617.569549	55.740724
2825.631003	191347.727783	55.745729
2824.654014	191094.413895	55.750733
2824.260950	190839.303998	55.755738
2823.658718	190571.276689	55.760743
2822.768045	190314.505350	55.765748
2822.521109	190053.714851	55.770753
2821.492439	189804.131019	55.775757
2820.866368	189538.390655	55.780762
2820.444031	189276.868847	55.785767
2819.667403	189021.040643	55.790772
2818.672716	188767.665619	55.795777
2818.275759	188509.719052	55.800781
2817.476447	188255.679746	55.805786
2816.827098	187991.389444	55.810791
2816.343808	187730.076766	55.815796
2815.639718	187464.716755	55.820801
2814.958528	187216.084026	55.825805
2814.169735	186941.758732	55.830810
2813.611588	186691.684503	55.835815
2812.764517	186431.060177	55.840820
2812.499655	186170.523245	55.845825
2811.959318	185919.814343	55.850829
2811.163278	185657.761546	55.855834
2810.418232	185397.457753	55.860839
2809.696570	185137.469795	55.865844
2809.189252	184868.735298	55.870849
2808.082605	184623.389907	55.875853
2807.698378	184352.501847	55.880858
2807.262295	184093.098065	55.885863
2806.188133	183830.540264	55.890868
2805.783298	183573.335306	55.895873
2804.943896	183306.838107	55.900877
2804.450229	183042.539347	55.905882
2803.990296	182786.696106	55.910887
2803.349062	182522.792745	55.915892
2802.468077	182252.873960	55.920897
2802.008845	182001.627325	55.925901
2801.204993	181733.353211	55.930906
2800.440310	181467.809425	55.935911
2799.713515	181214.459991	55.940916
2799.087172	180953.743876	55.945921
2798.427796	180693.556098	55.950925
2797.524023	180431.271641	55.955930
2796.986674	180178.050964	55.960935
2796.071373	179921.342802	55.965940
2795.690726	179660.163192	55.970945
2794.722631	179408.859683	55.975949
2794.070210	179148.209619	55.980954
2793.621231	178893.405384	55.985959
2792.972383	178633.622870	55.990964
2792.265706	178371.192767	55.995969
2791.658867	178114.853775	56.000973
2791.011901	177862.898133	56.005978
2790.628145	177599.569553	56.010983
2789.639739	177344.008011	56.015988
2789.402545	177078.039401	56.020993
2788.342937	176827.567212	56.025997
2787.980208	176561.863472	56.031002
2787.463363	176287.066504	56.036007
2786.417751	176039.242412	56.041012
2786.097995	175784.920128	56.046017
2785.312508	175506.571591	56.051021
2784.621325	175249.589714	56.056026
2783.885836	174994.549673	56.061031
2783.114735	174737.685450	56.066036
2782.745531	174464.276436	56.071041
2782.035091	174211.424911	56.076045
2781.364720	173949.271756	56.081050
2780.864211	173688.021826	56.086055
2780.273917	173422.400164	56.091060
2779.536043	173152.848421	56.096065
2778.745152	172889.665748	56.101069
2778.315201	172619.318521	56.106074
2777.583965	172351.640669	56.111079
2776.786322	172092.444962	56.116084
2775.976099	171823.486035	56.121089
2775.266305	171565.971300	56.126093
2774.519312	171293.368867	56.131098
2774.082823	171022.931936	56.136103
2773.263701	170775.638839	56.141108
2772.669981	170498.986410	56.146113
2772.349341	170241.075458	56.151117
2771.154451	169982.109318	56.156122
2770.541472	169727.134806	56.161127
2770.139640	169471.912363	56.166132
2769.462716	169192.866347	56.171137
2768.663289	168962.799894	56.176141
2767.984487	168624.563520	56.181146
2767.462364	168334.754006	56.186151
2766.795013	168077.586510	56.191156
2765.969675	167806.585325	56.196161
2765.335174	167544.787625	56.201165
2764.595523	167286.250940	56.206170
2764.007747	167029.510334	56.211175
2763.316500	166773.487237	56.216180
2762.999815	166510.896195	56.221185
2762.462089	166241.640951	56.226189
2761.559331	165982.706794	56.231194
2761.175485	165708.446609	56.236199
2760.277873	165441.733655	56.241204
2759.496526	165176.237582	56.246209
2758.770296	164914.358477	56.251213
2758.331079	164641.284783	56.256218
2757.878436	164386.677200	56.261223
2756.764909	164113.739672	56.266228
2756.240789	163850.246827	56.271233
2755.563836	163577.040740	56.276237
2754.613108	163324.452086	56.281242
2754.412486	163052.140812	56.286247
2753.232922	162792.205068	56.291252
2752.466998	162521.602048	56.296257
2752.069098	162275.595416	56.301261
2751.201568	162007.923891	56.306266
2750.794216	161751.179019	56.311271
2750.066903	161484.773309	56.316276
2749.976443	161209.763238	56.321281
2748.583375	160964.444525	56.326285
2748.291618	160697.390903	56.331290
2747.750595	160424.492452	56.336295
2747.134059	160176.399103	56.341300
2746.541876	159905.826601	56.346305
2745.612948	159627.859610	56.351309
2744.653165	159356.548639	56.356314
2743.901876	159117.141717	56.361319
2743.315147	158832.071155	56.366324
2742.767166	158598.585214	56.371329
2741.571270	158321.611664	56.376333
2741.415379	158036.733642	56.381338
2740.691162	157818.383414	56.386343
2739.986068	157544.122390	56.391348
2739.120165	157295.453451	56.396353
2738.670092	157031.465800	56.401357
2738.177876	156784.966006	56.406362
2737.747804	156521.385906	56.411367
2737.181815	156257.587844	56.416372
2736.471603	155994.882462	56.421377
2736.118198	155727.317565	56.426381
2735.087060	155460.243478	56.431386
2734.182304	155190.304103	56.436391
2733.957951	154936.504305	56.441396
2733.304240	154658.406828	56.446401
2732.290331	154392.215557	56.451405
2731.522439	154129.864322	56.456410
2731.197994	153852.916217	56.461415
2730.390188	153602.180601	56.466420
2729.891270	153328.937938	56.471425
2729.312451	153060.845303	56.476429
2728.483527	152807.043041	56.481434
2727.897307	152542.031745	56.486439
2727.030714	152268.881487	56.491444
2726.396550	151996.954997	56.496449
2725.627260	151733.034162	56.501453
2725.089932	151485.449312	56.506458
2724.655894	151203.545693	56.511463
2723.761093	150945.612075	56.516468
2722.979540	150675.867879	56.521473
2722.313356	150414.279970	56.526477
2721.302395	150153.816389	56.531482
2720.756926	149886.024057	56.536487
2720.284774	149638.722550	56.541492
2720.067392	149371.924681	56.546497
2719.286129	149099.283164	56.551501
2718.482349	148842.597397	56.556506
2717.999429	148562.135241	56.561511
2717.007662	148310.872113	56.566516
2716.497635	148043.928312	56.571521
2716.033729	147772.264539	56.576525
2715.192188	147513.943320	56.581530
2714.622281	147240.636069	56.586535
2713.966255	146993.193541	56.591540
2713.055619	146694.871469	56.596545
2712.673660	146446.296911	56.601549
2711.809561	146172.079704	56.606554
2711.359798	145898.447362	56.611559
2710.567755	145658.534533	56.616564
2710.162123	145357.514669	56.621569
2709.198545	145129.438499	56.626573
2708.465163	144830.114924	56.631578
2707.967670	144598.131173	56.636583
2707.015385	144305.366209	56.641588
2706.843488	144051.783517	56.646593
2705.871409	143774.618366	56.651597
2705.060483	143520.785471	56.656602
2704.670048	143224.345715	56.661607
2703.999856	143000.978417	56.666612
2703.016296	142711.181528	56.671617
2702.951722	142432.194775	56.676621
2701.531025	142205.254604	56.681626
2701.423865	141922.518180	56.686631
2700.407630	141660.969746	56.691636
2700.011882	141381.384375	56.696641
2699.079859	141133.206599	56.701645
2698.295506	140875.528939	56.706650
2697.901018	140603.446997	56.711655
2697.185001	140355.622579	56.716660
2696.386121	140085.527930	56.721665
2695.677491	139830.286691	56.726669
2695.332079	139560.912673	56.731674
2694.652306	139287.642758	56.736679
2693.740784	139039.796693	56.741684
2693.438395	138771.020138	56.746689
2692.657945	138483.696525	56.751693
2691.865728	138258.058774	56.756698
2691.395114	137967.324352	56.761703
2690.396189	137710.394091	56.766708
2689.623165	137445.680639	56.771713
2689.350179	137189.376782	56.776717
2688.403100	136942.239990	56.781722
2687.835036	136676.421162	56.786727
2687.078108	136405.515004	56.791732
2685.996758	136154.531463	56.796737
2685.953882	135882.183156	56.801741
2685.055526	135638.937015	56.806746
2684.457128	135344.577579	56.811751
2683.680288	135118.288342	56.816756
2683.128299	134830.037093	56.821761
2682.440651	134578.229949	56.826765
2681.829239	134327.416465	56.831770
2681.598978	134062.165149	56.836775
2680.335683	133793.205602	56.841780
2680.230275	133538.584252	56.846785
2679.350327	133263.141434	56.851789
2678.279179	133001.208799	56.856794
2677.845788	132749.390171	56.861799
2677.358252	132485.667725	56.866804
2676.352608	132222.220342	56.871809
2675.628472	131966.275758	56.876813
2675.144778	131718.043507	56.881818
2674.771485	131465.375759	56.886823
2673.842000	131173.626729	56.891828
2673.513138	130943.832160	56.896833
2672.877310	130653.070836	56.901837
2671.759650	130420.382608	56.906842
2671.606698	130125.727199	56.911847
2670.648451	129878.856516	56.916852
2670.119008	129602.288982	56.921857
2669.479190	129336.397600	56.926861
2668.977224	129087.721660	56.931866
2668.680181	128804.736848	56.936871
2667.536164	128544.419561	56.941876
2667.146118	128283.997984	56.946881
2666.046943	128011.499093	56.951885
2665.328481	127752.087090	56.956890
2664.843370	127471.647672	56.961895
2664.463468	127230.944683	56.966900
2663.462719	126969.044867	56.971905
2663.046138	126674.963355	56.976909
2662.003200	126433.800963	56.981914
2661.859682	126149.942971	56.986919
2661.009394	125882.416707	56.991924
2659.988870	125631.746246	56.996929
2659.612325	125354.054435	57.001933
2658.692668	125092.096395	57.006938
2658.185011	124823.332653	57.011943
2657.311463	124581.702796	57.016948
2656.984941	124297.118664	57.021953
2655.843383	124039.536193	57.026957
2655.391570	123777.605746	57.031962
2654.936505	123518.103703	57.036967
2654.020676	123252.290147	57.041972
2653.402614	122986.165416	57.046977
2653.051138	122741.295058	57.051981
2652.131044	122463.186058	57.056986
2651.695739	122205.077736	57.061991
2651.421520	121940.216863	57.066996
2650.425796	121662.763130	57.072001
2649.919026	121414.018955	57.077005
2649.153574	121143.339814	57.082010
2648.674233	120861.813206	57.087015
2647.789670	120593.799531	57.092020
2646.928501	120343.572672	57.097025
2646.750382	120045.209678	57.102029
2645.878222	119785.353393	57.107034
2645.260874	119527.624015	57.112039
2644.561893	119253.964001	57.117044
2643.796045	118984.576919	57.122049
2643.052127	118704.512091	57.127053
2642.029889	118449.828379	57.132058
2641.875810	118195.206412	57.137063
2640.858865	117911.860898	57.142068
2640.158063	117661.044214	57.147073
2639.938265	117388.299253	57.152077
2638.779303	117111.046966	57.157082
2638.116008	116866.033694	57.162087
2637.802161	116575.520573	57.167092
2636.912074	116338.564965	57.172097
2636.252400	116049.267840	57.177101
2635.681316	115826.719007	57.182106
2635.209261	115518.617051	57.187111
2634.141442	115284.911051	57.192116
2633.611712	115017.254729	57.197121
2632.830039	114736.293720	57.202125
2632.506129	114486.730702	57.207130
2631.705747	114224.114269	57.212135
2630.921038	113958.419970	57.217140
2630.421034	113680.186938	57.222145
2629.739984	113428.983794	57.227149
2629.061987	113166.276559	57.232154
2628.614122	112889.192783	57.237159
2627.706722	112627.885698	57.242164
2627.127661	112359.910193	57.247169
2626.536640	112095.036415	57.252173
2625.694293	111841.615614	57.257178
2625.165611	111573.075831	57.262183
2624.771678	111306.332568	57.267188
2623.857030	111035.403895	57.272193
2623.115889	110770.777521	57.277197
2622.556033	110516.316594	57.282202
2621.762008	110241.690662	57.287207
2621.159882	109965.527142	57.292212
2620.292566	109712.449520	57.297217
2619.970520	109441.362077	57.302221
2618.899493	109187.719354	57.307226
2618.388735	108916.496326	57.312231
2617.952647	108644.192139	57.317236
2617.275072	108391.618504	57.322241
2616.555548	108109.967949	57.327245
2615.666344	107848.175942	57.332250
2615.193548	107595.831975	57.337255
2614.737138	107318.038464	57.342260
2613.597967	107049.423168	57.347265
2612.934202	106807.269531	57.352269
2612.330456	106536.779552	57.357274
2611.619230	106267.026605	57.362279
2610.826939	106011.818676	57.367284
2610.061590	105762.744369	57.372289
2609.583321	105496.205276	57.377293
2608.914268	105236.443486	57.382298
2608.468138	104970.666516	57.387303
2607.673187	104718.277070	57.392308
2606.766595	104464.176040	57.397313
2606.485891	104198.762167	57.402317
2605.673806	103928.544217	57.407322
2605.207463	103667.130764	57.412327
2604.379994	103419.613489	57.417332
2603.934472	103140.433315	57.422337
2602.972597	102890.659133	57.427341
2602.471102	102631.831994	57.432346
2601.816341	102348.615411	57.437351
2600.890711	102126.571607	57.442356
2600.409280	101836.736472	57.447361
2599.753151	101583.153455	57.452365
2599.180632	101332.452517	57.457370
2598.671269	101066.177895	57.462375
2598.390654	100799.426060	57.467380
2597.618929	100526.367596	57.472385
2596.940411	100259.799210	57.477389
2595.798849	100001.997149	57.482394
2595.005257	99717.667571	57.487399
2594.635753	99464.201907	57.492404
2593.495186	99206.808200	57.497409
2592.993126	98949.544542	57.502413
2592.293306	98692.771778	57.507418
2592.042907	98437.852472	57.512423
2591.100929	98170.620699	57.517428
2590.352763	97909.519813	57.522433
2590.365295	97644.242292	57.527437
2589.560507	97380.074085	57.532442
2588.792901	97118.408220	57.537447
2588.018991	96863.798793	57.542452
2587.364303	96585.010208	57.547457
2586.853164	96324.035878	57.552461
2586.017617	96055.201308	57.557466
2585.451474	95785.585266	57.562471
2584.766179	95530.672434	57.567476
2583.930500	95257.059420	57.572481
2583.362936	94999.629010	57.577485
2582.688315	94746.086843	57.582490
2582.505764	94471.022851	57.587495
2581.800775	94202.804915	57.592500
2580.985920	93938.355310	57.597505
2580.603650	93669.287314	57.602509
2579.883765	93405.513844	57.607514
2578.974660	93126.199879	57.612519
2578.166351	92861.254778	57.617524
2577.487141	92598.454637	57.622529
2577.065518	92328.965283	57.627533
2575.910998	92066.107302	57.632538
2575.505068	91801.637434	57.637543
2574.873903	91532.400270	57.642548
2574.245166	91268.251111	57.647553
2573.712556	90999.252148	57.652557
2573.176643	90728.380267	57.657562
2572.440742	90464.555779	57.662567
2571.504594	90199.415749	57.667572
2570.884219	89932.643872	57.672577
2570.379505	89658.952625	57.677581
2569.450192	89403.508795	57.682586
2568.829701	89117.536837	57.687591
2568.061096	88864.521084	57.692596
2567.816806	88596.723351	57.697601
2566.984179	88326.220042	57.702605
2565.849007	88079.896506	57.707610
2565.566861	87791.257547	57.712615
2564.860317	87534.348763	57.717620
2564.291355	87276.717579	57.722625
2563.403808	87010.011429	57.727629
2562.955900	86751.676388	57.732634
2562.188189	86481.109947	57.737639
2561.517021	86212.560121	57.742644
2560.918380	85961.763930	57.747649
2560.045023	85688.618968	57.752653
2559.396268	85426.801041	57.757658
2558.780859	85164.518329	57.762663
2558.327826	84900.222793	57.767668
2557.369971	84643.775294	57.772673
2557.088743	84367.561699	57.777677
2556.344622	84115.130691	57.782682
2555.568819	83843.768807	57.787687
2554.758313	83579.324602	57.792692
2554.105689	83324.676518	57.797697
2553.403255	83065.425285	57.802701
2552.681942	82802.878145	57.807706
2552.596573	82535.866678	57.812711
2551.719248	82281.361944	57.817716
2550.854357	82019.291039	57.822721
2550.355455	81747.608187	57.827725
2549.628978	81479.159097	57.832730
2548.983512	81212.468801	57.837735
2548.467142	80947.250769	57.842740
2547.873621	80681.319556	57.847745
2547.169320	80419.338428	57.852749
2546.344240	80158.317664	57.857754
2545.692907	79884.287900	57.862759
2544.922318	79624.551684	57.867764
2544.254281	79361.456574	57.872769
2544.030354	79088.586350	57.877773
2542.788341	78843.135653	57.882778
2542.148977	78574.780191	57.887783
2541.686450	78307.490119	57.892788
2541.413388	78037.765619	57.897793
2540.585566	77770.964999	57.902797
2539.585617	77508.497553	57.907802
2538.999867	77242.140716	57.912807
2538.116042	76975.150294	57.917812
2537.195329	76710.266487	57.922817
2536.971269	76451.396358	57.927821
2536.335228	76194.958145	57.932826
2535.897270	75933.651162	57.937831
2534.794800	75676.463443	57.942836
2533.999664	75415.270460	57.947841
2533.310013	75145.010501	57.952845
2532.516413	74899.023191	57.957850
2532.266571	74642.334428	57.962855
2531.650701	74382.906705	57.967860
2530.800783	74117.811305	57.972865
2530.351213	73866.010651	57.977869
2529.420942	73605.711543	57.982874
2528.865542	73342.885733	57.987879
2528.238330	73088.791720	57.992884
2527.420712	72838.601759	57.997889
2526.915217	72570.235177	58.002893
2525.789433	72327.252518	58.007898
2525.407652	72060.349215	58.012903
2524.686941	71800.344574	58.017908
2524.129105	71548.134312	58.022913
2523.614225	71287.761721	58.027917
2522.380149	71038.788010	58.032922
2521.862304	70786.049058	58.037927
2521.327549	70539.548862	58.042932
2520.729605	70283.091894	58.047937
2520.123593	70015.098977	58.052941
2519.525929	69780.747909	58.057946
2518.641937	69517.404291	58.062951
2518.033766	69262.710431	58.067956
2517.091879	69017.060285	58.072961
2516.658269	68761.825925	58.077965
2515.807344	68509.086787	58.082970
2515.098098	68258.089171	58.087975
2514.460683	68008.964418	58.092980
2514.050008	67761.529574	58.097985
2513.577759	67499.819948	58.102989
2512.357906	67253.244993	58.107994
2511.867862	67009.755692	58.112999
2511.360581	66753.612613	58.118004
2510.448913	66503.546919	58.123009
2509.993883	66250.176038	58.128013
2509.229728	66002.389102	58.133018
2508.768961	65746.464180	58.138023
2508.465766	65503.825522	58.143028
2507.505528	65243.591684	58.148033
2506.925111	64989.484739	58.153037
2505.953306	64746.796996	58.158042
2505.520998	64484.675598	58.163047
2505.242805	64234.817681	58.168052
2504.510491	63988.251691	58.173057
2503.885217	63725.218341	58.178061
2502.997642	63471.898963	58.183066
2502.211797	63205.782972	58.188071
2501.624140	62954.566265	58.193076
2500.732977	62701.710454	58.198081
2500.614067	62436.291005	58.203085
2499.742896	62183.799844	58.208090
2499.226829	61929.194919	58.213095
2498.412287	61670.338644	58.218100
2497.561911	61421.387241	58.223105
2496.915660	61161.444485	58.228109
2496.250617	60911.223235	58.233114
2495.788740	60662.087361	58.238119
2495.008544	60406.262908	58.243124
2494.057069	60154.834153	58.248129
2493.545226	59894.504648	58.253133
2492.842926	59653.871745	58.258138
2491.887797	59399.256797	58.263143
2491.419716	59152.677387	58.268148
2490.413896	58906.730888	58.273153
2489.908324	58655.064936	58.278157
2489.493789	58413.661814	58.283162
2489.062269	58162.354788	58.288167
2488.175544	57910.449180	58.293172
2487.157529	57657.393615	58.298177
2487.241012	57404.258701	58.303181
2486.238408	57167.259834	58.308186
2485.566128	56908.735148	58.313191
2484.979060	56653.662852	58.318196
2484.294439	56408.847480	58.323201
2483.690535	56158.664747	58.328205
2482.720300	55911.439148	58.333210
2482.478434	55656.693080	58.338215
2481.900138	55411.494413	58.343220
2480.703033	55156.030146	58.348225
2480.503565	54900.202461	58.353229
2479.425962	54648.767391	58.358234
2478.751109	54401.717918	58.363239
2478.091757	54154.947804	58.368244
2477.339513	53902.003221	58.373249
2476.790101	53664.357689	58.378253
2476.230627	53418.205113	58.383258
2475.746105	53169.155106	58.388263
2475.119837	52929.183580	58.393268
2474.020791	52687.192388	58.398273
2473.656441	52423.635740	58.403277
2473.184987	52182.317534	58.408282
2472.429869	51935.662465	58.413287
2471.749633	51673.087579	58.418292
2470.659169	51438.777964	58.423297
2470.056169	51190.485941	58.428301
2469.331133	50947.677394	58.433306
2468.816516	50692.395787	58.438311
2468.322476	50450.952568	58.443316
2467.375160	50204.861126	58.448321
2467.012722	49955.959658	58.453325
2466.387642	49716.777483	58.458330
2465.249112	49474.111456	58.463335
2464.596288	49221.343512	58.468340
2464.191131	48979.672033	58.473345
2463.331192	48726.279643	58.478349
2462.544961	48489.372886	58.483354
2461.985799	48252.882493	58.488359
2461.462826	48007.823403	58.493364
2460.434051	47771.480319	58.498369
2460.253790	47523.529882	58.503373
2459.293109	47285.926727	58.508378
2458.686996	47049.965986	58.513383
2458.241541	46809.383868	58.518388
2457.254941	46572.322686	58.523393
2456.920625	46336.515052	58.528397
2456.011794	46088.535857	58.533402
2455.221606	45846.462265	58.538407
2454.644109	45592.810811	58.543412
2453.886227	45373.065073	58.548417
2453.448591	45125.050141	58.553421
2452.640330	44892.262638	58.558426
2451.959358	44647.272341	58.563431
2450.999934	44414.758707	58.568436
2450.193071	44186.759129	58.573441
2450.023888	43938.946237	58.578445
2449.099331	43705.513111	58.583450
2448.593284	43464.300422	58.588455
2447.837668	43238.066669	58.593460
2446.923491	43010.188123	58.598465
2446.759080	42765.784464	58.603469
2445.921101	42535.604258	58.608474
2445.072853	42307.866833	58.613479
2444.556871	42069.865877	58.618484
2444.014642	41843.512226	58.623489
2443.178674	41602.817391	58.628493
2442.604612	41377.205373	58.633498
2441.780550	41132.240144	58.638503
2440.924958	40913.183127	58.643508
2439.835562	40690.246761	58.648513
2439.425628	40449.116412	58.653517
2438.775056	40219.457682	58.658522
2437.955598	40000.065157	58.663527
2437.460189	39778.455112	58.668532
2436.647206	39559.892446	58.673537
2435.803993	39324.019269	58.678541
2435.083788	39113.027766	58.683546
2434.693950	38892.732503	58.688551
2434.018923	38669.551385	58.693556
2432.880201	38467.085108	58.698561
2432.378466	38242.600142	58.703565
2432.050008	38031.820808	58.708570
2431.332574	37802.922984	58.713575
2430.630772	37589.095963	58.718580
2429.839330	37379.850804	58.723585
2429.592497	37151.031053	58.728589
2428.559521	36935.907051	58.733594
2427.775950	36729.136071	58.738599
2427.271221	36509.229923	58.743604
2426.254571	36301.900532	58.748609
2425.729791	36078.015464	58.753613
2424.999230	35865.326030	58.758618
2423.900652	35652.174497	58.763623
2423.600303	35446.975365	58.768628
2422.689748	35255.804068	58.773633
2422.380090	35044.717819	58.778637
2421.272966	34830.808446	58.783642
2420.715939	34635.200968	58.788647
2420.211051	34427.466000	58.793652
2419.172346	34225.534419	58.798657
2418.888900	34014.746264	58.803661
2417.769019	33822.719064	58.808666
2417.108859	33621.553416	58.813671
2416.274939	33426.209500	58.818676
2415.474735	33241.654184	58.823681
2415.110594	33037.545742	58.828685
2413.980849	32849.899187	58.833690
2412.865885	32666.741803	58.838695
2412.364125	32481.199529	58.843700
2410.849366	32318.934792	58.848705
2409.827425	32156.719933	58.853709
2409.064620	31990.554722	58.858714
2408.119100	31824.423316	58.863719
2407.458697	31669.955467	58.868724
2406.118745	31531.606412	58.873729
2405.826067	31378.610959	58.878733
2404.613332	31252.483462	58.883738
2403.599824	31106.939545	58.888743
2403.134246	30974.114769	58.893748
2402.259125	30851.975436	58.898753
2401.871956	30709.077114	58.903757
2401.045465	30594.498730	58.908762
2400.645617	30465.819929	58.913767
2399.610607	30334.163446	58.918772
2398.939719	30213.153052	58.923777
2398.197643	30083.168001	58.928781
2397.515722	29957.644133	58.933786
2396.705024	29838.549884	58.938791
2396.036818	29730.371766	58.943796
2395.284255	29615.055446	58.948801
2394.682320	29488.950572	58.953805
2393.876017	29376.971741	58.958810
2393.199643	29264.949383	58.963815
2392.865295	29160.779259	58.968820
2392.000039	29057.545526	58.973825
2391.586566	28936.440602	58.978829
2391.010324	28819.545808	58.983834
2390.158566	28704.002059	58.988839
2389.573802	28597.530780	58.993844
2388.909000	28483.630407	58.998849
2388.443147	28370.059485	59.003853
2387.861382	28260.305544	59.008858
2387.123449	28146.643464	59.013863
2386.676356	28029.648576	59.018868
2385.688837	27914.308916	59.023873
2385.326670	27806.717509	59.028877
2384.919889	27696.129240	59.033882
2383.924563	27579.519152	59.038887
2383.158242	27461.425793	59.043892
2382.671035	27346.509257	59.048897
2382.040174	27236.220314	59.053901
2381.481311	27120.552969	59.058906
2380.785664	27009.102152	59.063911
2380.096178	26893.945261	59.068916
2379.522604	26798.083536	59.073921
2378.969768	26671.428085	59.078925
2378.223767	26556.329957	59.083930
2377.316575	26438.081617	59.088935
2377.191714	26325.813668	59.093940
2376.097727	26217.604115	59.098945
2375.617254	26086.284384	59.103949
2374.913252	25988.794350	59.108954
2374.515599	25868.806916	59.113959
2373.625236	25749.465558	59.118964
2372.949532	25644.725403	59.123969
2372.455425	25527.836689	59.128973
2372.019527	25410.836929	59.133978
2371.228124	25304.627867	59.138983
2370.601437	25183.110280	59.143988
2370.325656	25066.519638	59.148993
2369.477882	24938.917710	59.153997
2368.409605	24824.966622	59.159002
2367.737437	24708.665722	59.164007
2367.151512	24602.874934	59.169012
2366.591452	24495.378923	59.174017
2365.619879	24379.239248	59.179021
2364.981296	24257.676099	59.184026
2364.228694	24143.968853	59.189031
2363.886677	24041.560110	59.194036
2363.146398	23931.678457	59.199041
2362.576785	23804.330526	59.204045
2361.861251	23705.066853	59.209050
2361.665079	23590.321412	59.214055
2360.999137	23460.899684	59.219060
2359.777345	23354.793179	59.224065
2359.461870	23225.932934	59.229069
2359.081609	23117.155868	59.234074
2358.236621	23004.819337	59.239079
2357.652744	22868.514076	59.244084
2356.922249	22770.102737	59.249089
2356.511601	22636.174830	59.254093
2355.476257	22526.213881	59.259098
2354.759214	22419.307165	59.264103
2354.484660	22299.672927	59.269108
2353.503008	22186.461363	59.274113
2352.842982	22067.509836	59.279117
2352.381693	21942.879021	59.284122
2351.736638	21823.739036	59.289127
2351.176992	21711.356972	59.294132
2350.269017	21586.487132	59.299137
2349.612014	21471.102136	59.304141
2349.097780	21359.257018	59.309146
2348.294301	21250.963361	59.314151
2347.754666	21115.158100	59.319156
2347.031688	21009.820432	59.324161
2346.513868	20897.180552	59.329165
2345.493180	20772.636642	59.334170
2345.020447	20651.652033	59.339175
2344.367753	20546.022497	59.344180
2343.559356	20432.113544	59.349185
2342.843388	20314.943545	59.354189
2342.411160	20203.176942	59.359194
2341.197233	20091.054293	59.364199
2341.047801	19963.013458	59.369204
2340.289660	19859.803717	59.374209
2339.595775	19743.554626	59.379213
2339.052144	19629.479261	59.384218
2338.287119	19516.109693	59.389223
2337.645240	19403.517189	59.394228
2336.742755	19287.346805	59.399233
2336.188974	19178.053694	59.404237
2335.724798	19063.524616	59.409242
2334.868664	18967.075740	59.414247
2334.549860	18837.755780	59.419252
2333.419521	18735.868071	59.424257
2332.916535	18615.833542	59.429261
2332.248835	18501.818459	59.434266
2331.286569	18400.721752	59.439271
2331.154146	18279.410240	59.444276
2330.162586	18180.872915	59.449281
2329.882540	18068.412265	59.454285
2329.095927	17944.127708	59.459290
2328.177192	17834.566413	59.464295
2327.477400	17719.256533	59.469300
2326.941519	17614.759283	59.474305
2326.246608	17502.056723	59.479309
2325.408275	17391.227376	59.484314
2324.810881	17286.276771	59.489319
2324.439247	17172.729679	59.494324
2323.836438	17062.876874	59.499329
2323.352623	16946.957341	59.504333
2322.603044	16832.817532	59.509338
2321.860178	16735.990025	59.514343
2321.248416	16610.373631	59.519348
2320.538005	16498.103912	59.524353
2319.764761	16401.114805	59.529357
2319.003069	16275.388955	59.534362
2318.673168	16161.706909	59.539367
2317.662205	16060.251588	59.544372
2316.921557	15953.864385	59.549377
2316.339299	15846.652178	59.554381
2315.580978	15730.214767	59.559386
2314.571644	15630.074873	59.564391
2314.363160	15523.518445	59.569396
2313.501779	15414.641811	59.574401
2312.539106	15299.401354	59.579405
2311.916426	15197.896757	59.584410
2311.461419	15097.098355	59.589415
2310.737454	14996.086965	59.594420
2309.522574	14898.995053	59.599425
2309.200744	14813.713790	59.604429
2308.486159	14709.124994	59.609434
2307.955137	14604.890445	59.614439
2307.202598	14498.503763	59.619444
2306.566025	14402.480062	59.624449
2305.688249	14307.914487	59.629453
2305.301964	14217.289120	59.634458
2304.566267	14114.755064	59.639463
2304.219169	14012.837283	59.644468
2303.202666	13931.192790	59.649473
2302.529286	13831.032683	59.654477
2301.892465	13713.570626	59.659482
2300.713580	13623.255394	59.664487
2300.418648	13536.590725	59.669492
2299.821209	13443.139099	59.674497
2299.003430	13339.529011	59.679501
2298.536110	13255.591560	59.684506
2297.841419	13165.909223	59.689511
2297.630799	13058.272495	59.694516
2296.591576	12962.435740	59.699521
2295.880908	12864.511947	59.704525
2295.329478	12769.434529	59.709530
2294.503179	12672.537222	59.714535
2293.924714	12577.225996	59.719540
2293.363914	12495.110472	59.724545
2292.192859	12399.294824	59.729549
2291.432241	12307.794539	59.734554
2290.709353	12216.569737	59.739559
2290.558008	12123.403064	59.744564
2289.491391	12049.808611	59.749569
2289.277413	11961.021006	59.754573
2288.605185	11859.232719	59.759578
2287.517743	11782.255797	59.764583
2286.951819	11692.341986	59.769588
2286.267821	11604.660733	59.774593
2285.847741	11511.027358	59.779597
2285.161993	11430.377039	59.784602
2284.063307	11340.517067	59.789607
2283.694256	11241.992706	59.794612
2282.750453	11169.682209	59.799617
2281.971548	11081.007506	59.804621
2281.747737	10994.655555	59.809626
2280.848490	10915.410012	59.814631
2280.155457	10828.984893	59.819636
2279.429186	10741.739053	59.824641
2278.536641	10667.967898	59.829645
2277.945442	10593.316127	59.834650
2277.536319	10510.593198	59.839655
2276.954473	10418.030969	59.844660
2275.626548	10352.261371	59.849665
2275.175079	10275.656383	59.854669
2274.995045	10187.917634	59.859674
2274.035694	10118.662877	59.864679
2273.488699	10030.124840	59.869684
2272.927103	9948.733746	59.874689
2271.930464	9876.698988	59.879693
2271.230984	9785.761298	59.884698
2270.439579	9716.759472	59.889703
2270.134754	9636.467414	59.894708
2269.095458	9572.919354	59.899713
2268.682264	9497.035729	59.904718
2268.317024	9419.652600	59.909722
2267.069191	9352.508635	59.914727
2266.702498	9272.340760	59.919732
2265.741696	9200.385223	59.924737
2265.137311	9125.206759	59.929742
2264.662807	9045.489132	59.934746
2263.833909	8979.677576	59.939751
2263.364571	8899.630138	59.944756
2262.706638	8838.192253	59.949761
2261.697729	8756.781536	59.954766
2261.311320	8685.915209	59.959770
2260.559611	8619.277272	59.964775
2259.837518	8535.861067	59.969780
2259.315251	8464.878884	59.974785
2258.661615	8408.820737	59.979790
2257.816685	8330.535574	59.984794
2257.166069	8259.927353	59.989799
2256.848729	8190.537485	59.994804
2256.062332	8122.196591	59.999809
2255.224277	8048.499899	60.004814
2254.478463	7970.488054	60.009818
2253.791677	7914.140411	60.014823
2253.247090	7843.313030	60.019828
2252.682727	7774.990971	60.024833
2251.815044	7698.786632	60.029838
2251.228689	7630.092839	60.034842
2249.970489	7550.195504	60.039847
2250.072999	7507.499764	60.044852
2249.141162	7431.788159	60.049857
2248.372653	7373.863654	60.054862
2247.811083	7308.831542	60.059866
2247.085063	7252.070606	60.064871
2246.565867	7177.766796	60.069876
2245.676595	7116.236235	60.074881
2245.439435	7048.975874	60.079886
2244.687366	6984.898309	60.084890
2243.689734	6914.073849	60.089895
2243.274437	6844.003751	60.094900
2242.796947	6785.790852	60.099905
2241.813037	6724.153874	60.104910
2241.597535	6648.430455	60.109914
2240.748371	6582.972283	60.114919
2239.858801	6518.833351	60.119924
2239.110919	6456.572404	60.124929
2238.479733	6388.497250	60.129934
2237.968803	6330.429479	60.134938
2236.944989	6274.393136	60.139943
2236.489880	6201.648976	60.144948
2235.732730	6137.860625	60.149953
2234.894889	6087.129928	60.154958
2234.421395	6018.541640	60.159962
2234.034728	5957.559292	60.164967
2233.380740	5887.877837	60.169972
2232.753442	5833.300202	60.174977
2232.376051	5767.631198	60.179982
2231.936017	5693.914616	60.184986
2230.770341	5626.372599	60.189991
2230.288795	5560.646893	60.194996
2229.601784	5502.965231	60.200001
2228.697308	5434.694097	60.205006
2228.033842	5360.071301	60.210010
2226.894535	5305.668324	60.215015
2226.340200	5236.060896	60.220020
2225.644593	5190.810459	60.225025
2225.274411	5127.980169	60.230030
2224.622390	5066.619261	60.235034
2223.622843	5028.881886	60.240039
2223.251190	4962.675286	60.245044
2222.456114	4894.692953	60.250049
2221.791905	4831.228340	60.255054
2221.560530	4772.750873	60.260058
2220.826104	4716.469491	60.265063
2220.239114	4652.077731	60.270068
2219.373532	4592.364753	60.275073
2218.388521	4529.545419	60.280078
2218.146430	4464.851335	60.285082
2217.283529	4419.191304	60.290087
2216.918954	4340.417265	60.295092
2216.159094	4280.908823	60.300097
2215.116819	4241.869485	60.305102
2214.599662	4174.661089	60.310106
2213.789966	4116.433332	60.315111
2213.382099	4050.235003	60.320116
2212.558602	4000.449301	60.325121
2211.577556	3935.443370	60.330126
2211.270650	3877.881290	60.335130
2210.191595	3832.859900	60.340135
2209.732119	3778.737239	60.345140
2209.103517	3716.951597	60.350145
2208.611890	3671.619070	60.355150
2207.770987	3618.928940	60.360154
2207.105516	3565.601561	60.365159
2207.022340	3496.000975	60.370164
2206.109006	3446.382036	60.375169
2205.697435	3405.174752	60.380174
2205.428847	3326.388560	60.385178
2204.475304	3270.951873	60.390183
2203.950417	3200.548973	60.395188
2203.229399	3147.812344	60.400193
2202.625194	3088.415753	60.405198
2201.563638	3026.345256	60.410202
2200.968064	2963.240593	60.415207
2200.484132	2901.304538	60.420212
2199.017891	2842.893428	60.425217
2198.260444	2796.732808	60.430222
2198.137735	2729.647479	60.435226
2197.267271	2693.774065	60.440231
2197.022045	2633.897331	60.445236
2196.450217	2559.177242	60.450241
2195.442882	2497.377974	60.455246
2194.504104	2443.386754	60.460250
2193.797692	2398.544096	60.465255
2193.347989	2340.312044	60.470260
2192.455450	2299.878110	60.475265
2191.606454	2249.626132	60.480270
2191.664046	2189.472923	60.485274
2190.745267	2140.779536	60.490279
2190.025113	2095.579623	60.495284
2189.246706	2036.962492	60.500289
2188.402658	1987.977039	60.505294
2188.090141	1922.787280	60.510298
2186.991679	1887.492965	60.515303
2186.756198	1824.111374	60.520308
2186.338468	1776.734643	60.525313
2185.289604	1736.181199	60.530318
2184.845777	1670.338417	60.535322
2183.862594	1614.499550	60.540327
2183.166771	1569.295049	60.545332
2182.345633	1524.955862	60.550337
2181.878701	1476.045571	60.555342
2181.364868	1420.850544	60.560346
2180.338238	1384.719698	60.565351
2180.130981	1329.121555	60.570356
2179.274306	1266.296696	60.575361
2178.743905	1224.992207	60.580366
2178.586512	1183.048326	60.585370
2177.582077	1130.162901	60.590375
2176.914179	1070.767296	60.595380
2176.038771	1028.248622	60.600385
2175.335945	982.490386	60.605390
2174.712471	924.417727	60.610394
2173.745796	880.482074	60.615399
2173.139423	825.203067	60.620404
2172.356315	788.831652	60.625409
2171.535885	747.263874	60.630414
2170.747952	702.623893	60.635418
2170.174880	663.650622	60.640423
2169.778114	629.501735	60.645428
2168.986575	580.360536	60.650433
2168.431640	541.362640	60.655438
2168.029840	486.781014	60.660442
2167.223566	456.239279	60.665447
2166.702589	413.828609	60.670452
2165.907281	354.210157	60.675457
2164.836326	314.312321	60.680462
2164.052894	277.880746	60.685466
2163.442474	250.008036	60.690471
2162.756116	211.832945	60.695476
2162.020922	185.284249	60.700481
2161.162886	154.637830	60.705486
2160.834919	121.695012	60.710490
2159.786673	83.000534	60.715495
2159.395844	51.753535	60.720500
2158.447389	20.919905	60.725505
2157.454024	7.620413	60.730510
2156.454888	-29.977739	60.735514
2153.903993	4.058440	60.740519
2151.121820	67.398265	60.745524
2151.710355	53.450394	60.750529
2152.023385	64.032019	60.755534
2152.306815	44.621365	60.760538
2152.177237	58.502652	60.765543
2151.214839	50.113344	60.770548
2150.345706	60.704328	60.775553
2148.803337	69.196071	60.780558
2148.688188	61.842389	60.785562
2148.208297	69.544281	60.790567
2147.393168	61.948428	60.795572
2147.205580	62.700364	60.800577
2146.671164	76.939195	60.805582
2146.158319	67.852536	60.810586
2144.971917	83.368011	60.815591
2144.223490	66.410667	60.820596
2143.535329	80.377439	60.825601
2142.808339	72.111617	60.830606
2142.607024	66.230218	60.835610
2142.250981	75.894604	60.840615
2141.479934	80.760157	60.845620
2140.642493	71.482155	60.850625
2139.620246	81.553424	60.855630
2138.996810	69.824112	60.860634
2138.205984	69.137450	60.865639
2137.936695	75.211707	60.870644
2137.514085	70.387235	60.875649
2136.662378	81.513188	60.880654
2136.198061	79.398106	60.885658
2135.346255	75.097446	60.890663
2134.626610	78.213967	60.895668
2133.747211	74.576822	60.900673
2133.171866	79.816585	60.905678
2132.561645	73.673645	60.910682
2132.629296	66.238923	60.915687
2131.772724	66.696471	60.920692
2130.864654	70.984547	60.925697
2130.447916	77.872217	60.930702
2129.789681	60.938422	60.935706
2128.155624	71.500974	60.940711
2127.695765	62.049543	60.945716
2127.292569	71.503798	60.950721
2126.658697	73.174904	60.955726
2126.052514	61.578478	60.960730
2125.333474	70.707546	60.965735
2125.437685	72.723576	60.970740
2124.210197	59.087478	60.975745
2123.472570	82.051893	60.980750
2123.450437	59.127528	60.985754
2122.318267	70.696924	60.990759
2121.742429	73.634520	60.995764
2121.123682	61.778327	61.000769
2120.215704	65.404101	61.005774
2119.991633	69.110593	61.010778
2119.094584	73.023204	61.015783
2118.027586	68.203210	61.020788
2117.952074	59.442974	61.025793
2117.451518	67.433561	61.030798
2116.021900	61.499482	61.035802
2115.377891	74.863187	61.040807
2115.145553	63.048184	61.045812
2114.780977	62.051060	61.050817
2113.748332	74.437263	61.055822
2113.459937	65.882680	61.060826
2112.911974	76.518915	61.065831
2111.453845	66.467394	61.070836
2111.095465	66.694523	61.075841
2110.613107	73.960017	61.080846
2110.030947	77.195072	61.085850
2109.179592	76.186877	61.090855
2108.334236	71.708594	61.095860
2107.796335	62.141823	61.100865
2107.231362	74.890621	61.105870
2106.899712	67.678519	61.110874
2105.540703	75.248680	61.115879
2105.348410	65.753222	61.120884
2104.773573	60.419929	61.125889
2103.790099	70.109751	61.130894
2103.039885	64.917818	61.135898
2102.443778	73.122257	61.140903
2102.024522	63.375821	61.145908
2101.925693	61.278448	61.150913
2100.248493	63.499859	61.155918
2099.683016	70.822693	61.160922
2099.420612	74.677189	61.165927
2098.617504	69.864215	61.170932
2098.669439	66.270115	61.175937
2096.997780	80.102796	61.180942
2096.389085	62.530401	61.185946
2096.214931	62.975871	61.190951
2095.371378	72.091587	61.195956
2094.592168	66.014897	61.200961
2093.770856	70.746514	61.205966
2093.549637	62.088243	61.210970
2092.874934	59.768446	61.215975
2091.996268	65.384329	61.220980
2091.495237	65.504791	61.225985
2090.491871	83.028566	61.230990
2090.058601	66.516382	61.235994
2089.251282	68.785847	61.240999
2088.825952	63.938166	61.246004
2088.337661	66.590652	61.251009
2087.315618	68.809037	61.256014
2086.924211	63.687905	61.261018
2086.492946	74.699843	61.266023
2085.557618	66.487603	61.271028
2085.602563	65.373466	61.276033
2084.946192	75.853448	61.281038
2083.778165	77.379095	61.286042
2082.730306	67.024385	61.291047
2081.613898	62.675851	61.296052
2081.741037	63.563924	61.301057
2081.086037	75.734103	61.306062
2080.548332	60.414853	61.311066
2079.606118	76.408807	61.316071
2078.791657	69.642311	61.321076
2078.192142	66.955788	61.326081
2077.408696	67.439595	61.331086
2077.278693	61.488547	61.336090
2076.399783	60.762267	61.341095
2076.028026	63.314266	61.346100
2075.436782	66.189662	61.351105
2074.534480	75.989611	61.356110
2073.051435	60.651641	61.361114
2072.754542	65.722652	61.366119
2072.734996	66.947799	61.371124
2071.827776	63.657277	61.376129
2070.536735	67.230315	61.381134
2069.887768	65.972410	61.386138
2069.963334	60.840258	61.391143
2069.274401	65.289112	61.396148
2068.865079	64.325902	61.401153
2068.010287	74.506225	61.406158
2067.846531	58.003329	61.411162
2066.639630	68.154370	61.416167
2065.263829	68.708522	61.421172
2065.110379	61.528077	61.426177
2064.155299	74.729845	61.431182
2063.900785	67.973846	61.436186
2062.671579	68.340742	61.441191
2062.743695	74.662011	61.446196
2061.917323	61.780699	61.451201
2060.946236	66.234905	61.456206
2060.825550	80.471167	61.461210
2060.025146	72.513478	61.466215
2059.647507	63.473198	61.471220
2059.157283	67.333885	61.476225
2057.657849	73.954991	61.481230
2057.084485	61.071379	61.486234
2056.120812	77.401466	61.491239
2055.219538	68.376471	61.496244
2055.905582	61.288306	61.501249
2054.558588	78.808266	61.506254
2053.935154	56.424021	61.511258
2053.558624	71.281162	61.516263
2052.946115	69.744676	61.521268
2052.602803	67.307650	61.526273
2051.349345	71.535446	61.531278
2050.225914	57.633735	61.536282
2049.489026	68.202183	61.541287
2048.948369	70.005163	61.546292
2049.228256	56.915199	61.551297
2048.229010	64.901353	61.556302
2047.671637	60.254400	61.561306
2047.009756	65.009610	61.566311
2046.098922	65.571986	61.571316
2045.883103	68.165472	61.576321
2044.429983	75.244415	61.581326
2044.046392	67.185901	61.586330
2043.417003	63.867070	61.591335
2042.699647	71.690230	61.596340
2042.553843	57.324317	61.601345
2042.029218	67.903235	61.606350
2041.016949	53.944471	61.611354
2039.748192	58.449072	61.616359
2038.532783	64.399092	61.621364
2038.589544	60.939840	61.626369
2037.923016	64.697625	61.631374
2037.793784	52.650253	61.636378
2037.041064	61.128695	61.641383
2036.523521	62.254682	61.646388
2036.177232	58.156103	61.651393
2034.946500	65.557707	61.656398
2034.129215	60.966195	61.661402
2033.314729	67.095433	61.666407
2032.605491	57.085969	61.671412
2032.619819	50.615310	61.676417
2031.794531	60.038779	61.681422
2031.318138	62.403970	61.686426
2030.381783	64.399053	61.691431
2029.325104	56.163524	61.696436
2028.655318	58.070574	61.701441
2027.761272	72.629815	61.706446
2027.817230	64.771198	61.711450
2027.109480	62.521316	61.716455
2026.722641	56.338234	61.721460
2026.088568	56.494014	61.726465
2024.880891	64.612595	61.731470
2024.205243	66.708225	61.736474
2023.391853	62.538702	61.741479
2022.518426	63.353757	61.746484
2022.330745	58.260230	61.751489
2021.635270	65.491744	61.756494
2021.430228	62.405183	61.761498
2021.046817	54.789755	61.766503
2019.744306	60.859254	61.771508
2018.759593	68.944032	61.776513
2017.821944	63.053357	61.781518
2017.181998	52.228698	61.786522
2016.854672	53.116353	61.791527
2016.517530	60.153810	61.796532
2016.437059	52.140241	61.801537
2015.416667	64.474056	61.806542
2014.845296	57.553899	61.811546
2013.826557	58.054566	61.816551
2013.004500	60.252277	61.821556
2012.759131	60.341641	61.826561
2011.933116	69.793620	61.831566
2011.167404	64.517449	61.836570
2009.974229	68.921767	61.841575
2008.960942	71.182943	61.846580
2009.465409	63.492835	61.851585
2008.642876	57.727392	61.856590
2007.738129	56.913777	61.861594
2007.067667	59.997289	61.866599
2006.842285	55.362313	61.871604
2006.489160	53.008852	61.876609
2005.069657	62.092990	61.881614
2004.461541	58.576839	61.886618
2003.660795	65.325192	61.891623
2002.649465	61.573426	61.896628
2002.659984	61.492877	61.901633
2001.966798	71.007352	61.906638
2001.885738	62.653267	61.911642
2000.916982	63.568609	61.916647
1999.578857	60.329156	61.921652
1999.321288	70.838889	61.926657
1998.393801	64.697461	61.931662
1997.885130	48.231988	61.936666
1997.504951	61.361441	61.941671
1996.968241	60.595071	61.946676
1995.798814	65.329922	61.951681
1994.477887	67.878037	61.956686
1994.263092	57.823229	61.961690
1994.202964	55.139431	61.966695
1993.161881	61.060223	61.971700
1992.579928	60.966477	61.976705
1992.252903	60.236212	61.981710
1991.799258	53.253227	61.986714
1991.101230	63.954279	61.991719
1989.658591	55.371615	61.996724
1989.467505	52.390073	62.001729
1988.942984	58.120078	62.006734
1988.556674	59.392394	62.011738
1987.310575	58.303395	62.016743
1986.320743	62.647064	62.021748
1986.006684	60.981230	62.026753
1985.300358	60.624964	62.031758
1984.826317	60.285445	62.036762
1984.480475	63.175523	62.041767
1983.928932	65.647262	62.046772
1982.658774	55.599115	62.051777
1981.726597	69.188327	62.056782
1981.347992	55.078564	62.061786
1981.244289	56.134148	62.066791
1980.378081	71.318152	62.071796
1979.824875	50.794560	62.076801
1978.550079	72.123848	62.081806
1977.881740	58.493708	62.086810
1977.520731	58.850576	62.091815
1976.847125	60.682554	62.096820
1976.238824	58.875774	62.101825
1975.658041	60.227841	62.106830
1974.893208	53.917117	62.111834
1973.963941	61.926876	62.116839
1973.040038	63.686622	62.121844
1972.846102	51.975946	62.126849
1972.333007	62.286543	62.131854
1971.816957	56.522931	62.136858
1971.744360	59.666094	62.141863
1970.571165	60.456207	62.146868
1970.041749	48.792472	62.151873
1968.979149	63.290162	62.156878
1968.090047	63.445434	62.161882
1967.234666	62.966180	62.166887
1966.410066	54.476240	62.171892
1966.372236	62.248324	62.176897
1965.395009	58.923226	62.181902
1965.259952	56.429509	62.186906
1964.691928	55.333818	62.191911
1963.839733	66.876167	62.196916
1962.876553	58.488641	62.201921
1962.029550	55.951813	62.206926
1961.683361	58.206467	62.211930
1961.248724	51.222051	62.216935
1960.518016	50.625246	62.221940
1960.054578	53.652255	62.226945
1958.556647	59.566725	62.231950
1958.251590	50.584340	62.236954
1957.584486	60.763271	62.241959
1956.977786	56.657157	62.246964
1956.897782	64.804924	62.251969
1955.653518	52.013652	62.256974
1954.626277	58.563009	62.261978
1954.188281	51.096604	62.266983
1953.394383	65.955331	62.271988
1953.252170	58.128177	62.276993
1952.718050	61.164830	62.281998
1952.299927	54.736008	62.287002
1951.238222	63.716074	62.292007
1950.302050	56.885376	62.297012
1950.042148	63.588895	62.302017
1949.276144	59.262075	62.307022
1948.656718	61.411873	62.312026
1947.607588	58.230652	62.317031
1946.574833	56.406100	62.322036
1946.372335	52.120721	62.327041
1945.769329	58.680011	62.332046
1945.337182	57.340418	62.337050
1944.683588	60.219426	62.342055
1944.086571	60.206925	62.347060
1943.212287	46.863377	62.352065
1942.206781	64.830598	62.357070
1941.895382	56.169326	62.362074
1941.383414	58.712057	62.367079
1940.767565	51.135120	62.372084
1940.582641	63.203883	62.377089
1938.968517	63.639818	62.382094
1938.549522	59.216922	62.387098
1938.167506	56.681986	62.392103
1937.230680	58.445372	62.397108
1936.227149	55.425644	62.402113
1935.518274	54.946800	62.407118
1935.029262	56.367882	62.412122
1934.290936	51.948371	62.417127
1933.698278	53.493133	62.422132
1933.615826	55.406320	62.427137
1933.200934	67.208828	62.432142
1932.451210	50.806869	62.437146
1931.132798	51.676816	62.442151
1930.197824	62.536906	62.447156
1930.305622	45.199362	62.452161
1929.536408	60.842607	62.457166
1929.167858	49.771486	62.462170
1928.347601	48.734764	62.467175
1927.190374	53.272169	62.472180
1926.916572	48.719004	62.477185
1925.814315	64.008284	62.482190
1924.635713	49.279667	62.487194
1924.557939	54.076215	62.492199
1923.698606	61.228103	62.497204
1923.661252	48.368273	62.502209
1922.859497	56.085002	62.507214
1922.228503	62.860041	62.512218
1921.993106	52.434802	62.517223
1920.535404	57.776807	62.522228
1919.907307	52.705899	62.527233
1919.344396	52.855138	62.532238
1918.661786	56.916683	62.537242
1918.639310	52.650038	62.542247
1916.998343	44.945690	62.547252
1916.362053	48.577278	62.552257
1915.789117	58.955720	62.557262
1915.274483	51.980860	62.562266
1915.209175	59.066630	62.567271
1914.413413	65.244960	62.572276
1914.120518	51.678253	62.577281
1912.938341	58.080338	62.582286
1912.150212	47.731806	62.587290
1911.626740	51.055342	62.592295
1910.860761	50.118814	62.597300
1910.024972	47.249082	62.602305
1908.812752	61.866725	62.607310
1908.199019	51.298130	62.612314
1908.160414	55.907120	62.617319
1907.149971	58.066959	62.622324
1906.957580	54.741874	62.627329
1906.292076	71.574979	62.632334
1905.997257	62.816466	62.637338
1905.531079	61.546934	62.642343
1904.322684	67.312976	62.647348
1903.568308	53.835294	62.652353
1902.939518	63.624972	62.657358
1902.493600	63.424499	62.662362
1901.439269	52.454361	62.667367
1900.261152	59.089184	62.672372
1900.137312	63.352179	62.677377
1899.784412	59.191599	62.682382
1899.383778	53.895363	62.687386
1898.761593	59.309740	62.692391
1897.464641	57.397844	62.697396
1896.487242	50.695137	62.702401
1896.169971	58.554150	62.707406
1895.595394	57.845849	62.712410
1895.429363	45.731815	62.717415
1894.839219	53.671987	62.722420
1893.865659	53.008101	62.727425
1893.073486	57.664180	62.732430
1892.299458	57.869015	62.737434
1891.985947	64.404436	62.742439
1890.956055	67.570263	62.747444
1890.381882	56.320488	62.752449
1889.741113	58.202464	62.757454
1888.955766	62.510549	62.762458
1888.512591	59.466538	62.767463
1887.654617	63.641081	62.772468
1886.991999	58.805884	62.777473
1886.305639	62.558965	62.782478
1885.560345	63.479873	62.787482
1885.270417	60.449379	62.792487
1884.728917	63.225455	62.797492
1883.999534	54.991655	62.802497
1882.752892	59.847611	62.807502
1882.378138	66.457408	62.812506
1882.182927	62.475213	62.817511
1881.388481	64.449394	62.822516
1880.369320	48.982746	62.827521
1879.699391	59.633620	62.832526
1879.117575	66.258942	62.837530
1878.685052	60.193525	62.842535
1878.140980	61.301677	62.847540
1877.232723	60.215865	62.852545
1876.014968	62.476433	62.857550
1875.777059	60.956214	62.862554
1875.173193	64.912233	62.867559
1874.987663	62.462803	62.872564
1874.342378	62.577823	62.877569
1872.973011	57.438534	62.882574
1872.519737	61.679714	62.887578
1872.224456	60.577014	62.892583
1871.580897	63.697284	62.897588
1870.637751	49.560494	62.902593
1869.840372	64.167484	62.907598
1869.080430	61.892819	62.912602
1869.125079	57.390025	62.917607
1868.118583	62.704579	62.922612
1867.083538	59.623653	62.927617
1866.554796	64.958552	62.932622
1865.821684	61.894345	62.937626
1865.686581	63.972003	62.942631
1864.526176	66.002709	62.947636
1863.700161	53.717497	62.952641
1862.761847	67.815459	62.957646
1861.950660	57.352337	62.962650
1862.379694	48.029516	62.967655
1861.281655	66.393047	62.972660
1861.243963	55.321451	62.977665
1860.505166	59.667882	62.982670
1859.044902	56.154598	62.987674
1858.806803	53.719824	62.992679
1858.307635	52.258430	62.997684
1857.518615	48.701658	63.002689
1856.452416	56.845142	63.007694
1856.126031	49.395735	63.012698
1855.735795	43.470266	63.017703
1855.198232	54.142701	63.022708
1853.989666	57.704317	63.027713
1853.218536	53.217503	63.032718
1852.628883	56.321334	63.037722
1852.793018	53.122570	63.042727
1851.455234	54.591690	63.047732
1850.759715	50.698394	63.052737
1849.961352	54.516569	63.057742
1849.472196	54.111669	63.062746
1849.205092	40.884652	63.067751
1848.330256	60.387513	63.072756
1847.343515	55.285259	63.077761
1847.067379	56.371378	63.082766
1846.136252	57.876859	63.087770
1845.640026	48.290947	63.092775
1844.285696	52.528534	63.097780
1843.554277	52.674582	63.102785
1843.141611	62.117733	63.107790
1842.455417	50.379587	63.112794
1842.375022	52.366560	63.117799
1842.006876	55.346920	63.122804
1841.454431	59.397278	63.127809
1840.651830	57.891025	63.132814
1839.773515	54.742654	63.137818
1839.205532	53.722675	63.142823
1837.989660	58.602148	63.147828
1837.213756	54.636466	63.152833
1836.617127	60.944038	63.157838
1836.046556	61.998061	63.162842
1836.061673	57.421113	63.167847
1835.573409	64.449459	63.172852
1834.434188	49.069704	63.177857
1833.900233	61.241180	63.182862
1832.977142	60.036320	63.187866
1832.045772	51.473506	63.192871
1831.091162	56.973788	63.197876
1830.815449	51.244593	63.202881
1830.050266	51.006518	63.207886
1829.419019	65.629713	63.212890
1829.389814	53.536537	63.217895
1828.831807	57.376478	63.222900
1827.711363	58.431077	63.227905
1827.247055	52.851668	63.232910
1826.623981	52.620992	63.237914
1826.182033	51.125289	63.242919
1824.556968	57.663954	63.247924
1823.927070	46.635934	63.252929
1823.573548	49.308060	63.257934
1823.093624	55.586064	63.262938
1822.964230	50.940605	63.267943
1821.654621	46.236540	63.272948
1820.827876	50.994314	63.277953
1820.055390	50.082499	63.282958
1819.542961	50.252128	63.287962
1819.404743	55.249073	63.292967
1818.889483	62.822574	63.297972
1817.628769	56.267379	63.302977
1817.232984	55.800355	63.307982
1816.521320	60.446824	63.312986
1815.981947	51.063303	63.317991
1814.800642	44.935454	63.322996
1814.112142	52.457613	63.328001
1813.471146	52.092598	63.333006
1813.317097	60.551717	63.338010
1812.739780	59.525342	63.343015
1812.173772	52.568128	63.348020
1811.473620	47.898181	63.353025
1810.682871	52.336445	63.358030
1809.952712	57.681253	63.363034
1809.255255	43.967514	63.368039
1808.017753	52.767382	63.373044
1807.473875	55.236357	63.378049
1807.222524	57.460200	63.383054
1806.577351	52.273771	63.388058
1806.377047	45.592794	63.393063
1805.254530	51.301081	63.398068
1804.797919	48.481561	63.403073
1804.213887	45.239173	63.408078
1803.331850	44.961315	63.413082
1802.886665	49.723161	63.418087
1801.686577	56.044556	63.423092
1801.139138	52.747474	63.428097
1800.802746	51.947762	63.433102
1800.342784	51.115635	63.438106
1798.939436	48.780737	63.443111
1798.162366	43.796597	63.448116
1797.754100	48.013290	63.453121
1797.668098	47.957527	63.458126
1797.147537	51.862486	63.463130
1796.230950	47.387752	63.468135
1795.035777	49.458697	63.473140
1794.780337	52.312361	63.478145
1794.547735	52.289338	63.483150
1793.093698	49.703884	63.488154
1792.763685	52.954146	63.493159
1792.009330	55.905953	63.498164
1791.497429	59.163022	63.503169
1790.773240	57.477187	63.508174
1789.544180	52.485972	63.513178
1789.303215	52.084250	63.518183
1788.684531	65.361959	63.523188
1788.067169	57.979263	63.528193
1788.016949	55.970381	63.533198
1786.764946	60.895034	63.538202
1786.218767	45.201960	63.543207
1785.563051	56.757290	63.548212
1784.602639	53.483210	63.553217
1783.945279	46.390710	63.558222
1782.763963	61.834494	63.563226
1782.461602	57.435687	63.568231
1781.977048	49.790648	63.573236
1781.798518	59.936175	63.578241
1781.554270	57.686880	63.583246
1780.191296	57.286711	63.588250
1779.884572	50.176378	63.593255
1779.160335	61.094498	63.598260
1777.850522	52.337924	63.603265
1777.217851	52.671727	63.608270
1776.426823	55.332909	63.613274
1776.181360	41.876981	63.618279
1775.523271	48.389849	63.623284
1775.403894	43.563043	63.628289
1774.524038	45.227554	63.633294
1773.343379	64.771107	63.638298
1773.061325	42.697069	63.643303
1772.320276	53.638354	63.648308
1771.123629	48.296668	63.653313
1770.530388	36.204774	63.658318
1770.002183	56.196616	63.663322
1769.555073	41.642092	63.668327
1769.116609	48.820218	63.673332
1768.787365	47.257747	63.678337
1767.756193	39.410948	63.683342
1766.732801	49.643320	63.688346
1766.376727	47.689315	63.693351
1765.998359	50.283395	63.698356
1764.716721	48.157836	63.703361
1763.897194	48.702654	63.708366
1763.265335	52.254726	63.713370
1763.365561	43.107112	63.718375
1762.852063	49.562331	63.723380
1761.304316	42.053017	63.728385
1760.756163	53.137127	63.733390
1760.124667	51.184283	63.738394
1760.062399	41.945785	63.743399
1759.469569	39.876421	63.748404
1758.377518	50.985401	63.753409
1757.747544	46.742699	63.758414
1757.175735	47.044766	63.763418
1756.716444	39.192311	63.768423
1755.404760	52.245760	63.773428
1754.847057	48.601831	63.778433
1754.196391	37.797903	63.783438
1753.715145	52.031438	63.788442
1753.419851	51.324549	63.793447
1752.609047	47.457476	63.798452
1751.953393	56.664838	63.803457
1751.392897	48.568267	63.808462
1750.041456	42.330283	63.813466
1749.265051	42.966023	63.818471
1748.840340	42.461027	63.823476
1748.179440	44.718371	63.828481
1747.969598	45.775048	63.833486
1747.519424	52.139794	63.838490
1746.953272	35.849129	63.843495
1745.734185	50.529397	63.848500
1745.252110	46.160716	63.853505
1745.168605	51.076434	63.858510
1743.775928	47.707021	63.863514
1742.977678	46.670019	63.868519
1742.425854	57.824100	63.873524
1741.808691	49.826411	63.878529
1741.515158	57.683236	63.883534
1740.017233	52.151301	63.888538
1739.381200	49.751351	63.893543
1738.747071	48.823897	63.898548
1738.973941	53.602023	63.903553
1738.626172	45.389678	63.908558
1737.264497	51.112316	63.913562
1736.555194	51.545026	63.918567
1735.882023	50.095521	63.923572
1735.434070	56.884096	63.928577
1734.620103	53.613587	63.933582
1733.847468	43.070294	63.938586
1733.455364	48.574308	63.943591
1732.619122	52.955164	63.948596
1731.750169	44.100228	63.953601
1730.840753	46.816490	63.958606
1730.318898	39.995789	63.963610
1730.073086	56.418480	63.968615
1729.896204	63.540883	63.973620
1729.229017	51.828146	63.978625
1728.329912	49.517283	63.983630
1727.416871	65.221242	63.988634
1726.766151	56.557136	63.993639
1725.423368	53.104119	63.998644
1724.852411	45.472819	64.003649
1724.385189	46.067350	64.008654
1723.831802	48.507888	64.013658
1723.473106	44.472838	64.018663
1723.383996	54.790229	64.023668
1722.331944	47.375673	64.028673
1721.698738	47.031519	64.033678
1720.938530	58.803716	64.038682
1719.898321	50.881102	64.043687
1719.061069	41.369891	64.048692
1718.343862	45.834341	64.053697
1718.375968	50.320135	64.058702
1717.906034	50.082510	64.063706
1716.818302	43.318565	64.068711
1715.990913	54.330338	64.073716
1715.192769	52.126442	64.078721
1715.181305	52.990775	64.083726
1713.829345	56.770755	64.088730
1712.883532	43.307801	64.093735
1712.375199	52.781914	64.098740
1712.097701	53.221744	64.103745
1711.823464	54.315457	64.108750
1711.194303	56.618231	64.113754
1710.553197	45.937368	64.118759
1709.514160	45.060036	64.123764
1708.578437	51.170755	64.128769
1708.480343	44.027306	64.133774
1707.478328	49.251314	64.138778
1706.769066	43.010709	64.143783
1706.205007	54.885787	64.148788
1705.658727	52.260291	64.153793
1705.233703	50.564815	64.158798
1704.105212	49.752151	64.163802
1703.709927	50.253263	64.168807
1703.217647	55.349014	64.173812
1702.013382	54.356006	64.178817
1701.129812	45.557018	64.183822
1700.519442	53.653385	64.188826
1700.434455	45.932296	64.193831
1699.850938	56.243056	64.198836
1699.037034	48.837995	64.203841
1697.975383	45.674643	64.208846
1697.382501	52.782688	64.213850
1697.229517	43.027199	64.218855
1696.783338	52.907737	64.223860
1695.945989	48.103507	64.228865
1695.503091	51.154098	64.233870
1694.283727	58.219726	64.238874
1693.083582	49.236064	64.243879
1692.619534	58.236395	64.248884
1692.002386	59.252115	64.253889
1691.584396	43.852518	64.258894
1690.778971	55.376444	64.263898
1690.798353	48.670053	64.268903
1689.859671	47.018315	64.273908
1688.690768	44.217336	64.278913
1688.501771	55.474635	64.283918
1687.528060	55.324911	64.288922
1687.541528	44.524328	64.293927
1686.546621	55.365604	64.298932
1685.631330	51.262849	64.303937
1685.308041	42.836905	64.308942
1684.363037	53.928862	64.313946
1683.619473	48.244039	64.318951
1682.771690	48.801254	64.323956
1682.073827	56.559880	64.328961
1681.836921	38.476079	64.333966
1681.304943	53.485609	64.338970
1680.758903	53.752062	64.343975
1679.723492	58.281256	64.348980
1678.890219	52.427764	64.353985
1678.884469	56.448086	64.358990
1677.651127	54.452087	64.363994
1677.172112	45.182022	64.368999
1676.383107	56.192438	64.374004
1675.650031	48.356678	64.379009
1675.655367	49.875897	64.384014
1674.394285	57.009657	64.389018
1673.760139	49.093532	64.394023
1672.968407	52.454984	64.399028
1672.516177	59.187478	64.404033
1672.458006	45.670287	64.409038
1671.407709	53.577925	64.414042
1670.484409	59.271968	64.419047
1670.132639	47.438201	64.424052
1668.934588	46.783250	64.429057
1668.204896	45.688075	64.434062
1667.643757	44.045763	64.439066
1666.894545	43.947118	64.444071
1666.983563	50.440685	64.449076
1666.285174	57.248544	64.454081
1665.155534	49.948835	64.459086
1664.397423	49.679725	64.464090
1663.867422	54.954927	64.469095
1663.728330	49.070028	64.474100
1662.305956	41.573982	64.479105
1661.659744	48.915994	64.484110
1661.196505	53.735915	64.489114
1660.483573	40.360574	64.494119
1660.392933	51.187530	64.499124
1659.160135	56.071340	64.504129
1658.729053	46.364757	64.509134
1657.780447	51.372152	64.514138
1657.677582	52.757178	64.519143
1656.961778	54.324711	64.524148
1656.089162	59.812023	64.529153
1655.840436	47.898817	64.534158
1654.837447	60.136919	64.539162
1653.629996	50.306082	64.544167
1652.962625	53.720322	64.549172
1652.470263	42.426108	64.554177
1652.387160	44.326784	64.559182
1651.906539	56.264304	64.564186
1650.805322	52.064945	64.569191
1650.097274	54.984203	64.574196
1649.439491	62.540939	64.579201
1648.614433	50.728737	64.584206
1647.422153	59.009003	64.589210
1647.112742	37.149088	64.594215
1646.872480	49.723324	64.599220
1645.842235	57.366027	64.604225
1645.915246	49.563079	64.609230
1645.047120	50.214995	64.614234
1644.424453	55.558534	64.619239
1643.784983	52.807513	64.624244
1642.726115	49.167528	64.629249
1641.822924	46.428439	64.634254
1640.977517	55.572922	64.639258
1640.474456	51.855690	64.644263
1640.235262	44.185911	64.649268
1639.553375	38.619036	64.654273
1639.539617	39.239319	64.659278
1637.924177	45.628326	64.664282
1637.436063	36.679827	64.669287
1637.115964	37.883327	64.674292
1636.293025	42.235287	64.679297
1635.620088	47.993641	64.684302
1634.795408	47.539582	64.689306
1634.174214	46.991703	64.694311
1633.857610	39.804130	64.699316
1632.558849	53.019565	64.704321
1632.178854	51.162416	64.709326
1631.331891	45.976559	64.714330
1631.376214	48.695889	64.719335
1630.599086	45.203536	64.724340
1629.514161	49.504079	64.729345
1628.490713	42.070836	64.734350
1628.212432	60.100778	64.739354
1627.771063	53.699377	64.744359
1626.737710	48.243523	64.749364
1625.718530	53.014570	64.754369
1625.551386	43.710749	64.759374
1625.052175	42.943234	64.764378
1624.683487	53.189915	64.769383
1623.876611	54.439204	64.774388
1622.938006	57.076564	64.779393
1622.511665	47.192628	64.784398
1622.009308	54.935977	64.789402
1620.943748	52.364604	64.794407
1620.370363	53.409657	64.799412
1619.433901	60.291612	64.804417
1619.360625	58.515045	64.809422
1618.326162	65.396802	64.814426
1617.286635	48.276247	64.819431
1617.053508	50.115605	64.824436
1616.345352	50.970766	64.829441
1616.464433	60.947592	64.834446
1614.837627	52.649880	64.839450
1614.024840	48.031003	64.844455
1613.723206	53.023944	64.849460
1613.541132	56.424179	64.854465
1612.806294	41.194784	64.859470
1611.598974	49.734477	64.864474
1611.013400	44.453492	64.869479
1610.596031	50.231175	64.874484
1609.473542	40.855204	64.879489
1608.951586	48.541742	64.884494
1608.273137	47.317026	64.889498
1607.920512	48.822149	64.894503
1607.684652	47.369440	64.899508
1606.184968	44.181100	64.904513
1605.516769	46.706127	64.909518
1605.064032	49.561184	64.914522
1604.788951	58.462122	64.919527
1604.341676	38.756049	64.924532
1602.965633	52.057883	64.929537
1602.345443	45.232338	64.934542
1601.921685	34.015552	64.939546
1601.270997	52.904114	64.944551
1600.329758	45.473592	64.949556
1599.472729	52.103247	64.954561
1599.259640	50.959140	64.959566
1598.844674	55.012927	64.964570
1598.016155	39.580815	64.969575
1597.233515	36.645985	64.974580
1596.552506	57.400073	64.979585
1596.318207	49.884054	64.984590
1595.335396	48.338704	64.989594
1594.297166	38.832668	64.994599
1593.873780	50.075157	64.999604
1593.323014	60.500571	65.004609
1592.887519	45.367123	65.009614
1591.897887	49.844920	65.014618
1590.897326	53.498175	65.019623
1590.672726	46.832127	65.024628
1589.846801	57.361172	65.029633
1590.033585	45.478140	65.034638
1588.608238	49.834355	65.039642
1587.523641	52.264696	65.044647
1587.400752	47.416389	65.049652
1586.689825	50.832833	65.054657
1586.066378	45.945781	65.059662
1585.146523	57.205647	65.064666
1585.141460	47.765702	65.069671
1584.626646	48.493967	65.074676
1583.417364	39.872926	65.079681
1582.588655	33.564616	65.084686
1581.692531	43.688512	65.089690
1581.286636	52.711148	65.094695
1580.852617	29.808255	65.099700
1579.391776	41.497811	65.104705
1579.457990	47.050446	65.109710
1578.475761	44.182019	65.114714
1577.904962	53.372771	65.119719
1577.991718	48.918491	65.124724
1576.791327	41.819295	65.129729
1576.069382	35.303225	65.134734
1575.280729	47.874695	65.139738
1575.070214	43.508642	65.144743
1573.977757	46.206727	65.149748
1572.924679	46.394490	65.154753
1572.514270	41.796856	65.159758
1572.571209	51.458707	65.164762
1572.038952	37.693599	65.169767
1571.019951	30.991349	65.174772
1570.285959	38.426160	65.179777
1569.945008	46.610620	65.184782
1568.679720	41.675741	65.189786
1567.805825	40.611390	65.194791
1567.764796	37.221301	65.199796
1566.828834	48.844826	65.204801
1566.163583	47.805673	65.209806
1564.942857	49.934391	65.214810
1564.496226	44.356971	65.219815
1564.273356	51.283256	65.224820
1563.572984	43.852329	65.229825
1563.511028	41.739673	65.234830
1562.707383	41.110417	65.239834
1561.991915	44.144407	65.244839
1561.181885	38.296735	65.249844
1559.730322	50.522544	65.254849
1559.459333	39.070196	65.259854
1558.628343	43.267345	65.264858
1558.270239	33.388364	65.269863
1558.124720	41.130210	65.274868
1556.847600	45.590617	65.279873
1556.454570	36.469349	65.284878
1556.102264	51.973857	65.289882
1554.954501	44.292330	65.294887
1554.522218	32.550240	65.299892
1553.560381	45.628594	65.304897
1552.828000	39.580941	65.309902
1551.753310	37.977672	65.314906
1550.803400	36.737757	65.319911
1550.908507	33.642979	65.324916
1550.577650	47.098878	65.329921
1550.150522	35.018519	65.334926
1549.410517	39.306865	65.339930
1548.469833	40.260484	65.344935
1548.181518	47.641842	65.349940
1547.004410	48.503721	65.354945
1546.432406	36.736522	65.359950
1545.478694	40.070127	65.364954
1544.571588	42.350865	65.369959
1544.525379	33.778440	65.374964
1543.716945	46.780388	65.379969
1543.687368	35.365381	65.384974
1542.712070	47.835631	65.389978
1541.564440	43.847115	65.394983
1541.267697	45.390673	65.399988
1540.139941	45.461011	65.404993
1539.471063	41.416932	65.409998
1538.996876	47.287222	65.415002
1538.660691	36.567445	65.420007
1538.107550	36.634793	65.425012
1536.860229	41.549341	65.430017
1536.319294	46.108822	65.435022
1535.852712	52.892490	65.440026
1535.238123	44.862925	65.445031
1534.649532	48.986879	65.450036
1533.618613	50.822117	65.455041
1533.131245	41.299548	65.460046
1532.654499	44.871173	65.465050
1531.748230	40.420137	65.470055
1531.019683	33.083586	65.475060
1530.018775	45.371835	65.480065
1529.958715	30.473647	65.485070
1529.827392	39.102588	65.490074
1528.560435	47.803165	65.495079
1528.013470	50.370446	65.500084
1527.106521	43.890091	65.505089
1526.893184	35.839357	65.510094
1525.765448	45.990606	65.515098
1524.672821	38.350798	65.520103
1524.314801	44.002370	65.525108
1523.967222	49.978696	65.530113
1523.785529	40.557364	65.535118
1523.008589	49.484423	65.540122
1521.882451	42.980552	65.545127
1521.509158	40.739179	65.550132
1520.768431	48.212920	65.555137
1519.398361	39.421931	65.560142
1518.740585	36.713279	65.565146
1518.064375	53.246908	65.570151
1518.530599	36.301895	65.575156
1517.758582	45.885723	65.580161
1517.225061	43.668232	65.585166
1516.002234	43.417814	65.590170
1515.543867	40.959737	65.595175
1514.792006	42.380079	65.600180
1513.960903	52.113641	65.605185
1513.175776	32.551175	65.610190
1512.626382	42.613687	65.615194
1512.060990	45.258011	65.620199
1511.179069	39.506931	65.625204
1510.283609	49.933501	65.630209
1510.195117	39.015109	65.635214
1509.904648	41.707208	65.640218
1509.103282	45.541716	65.645223
1508.025378	36.901421	65.650228
1507.251794	58.879680	65.655233
1507.095873	40.242195	65.660238
1505.753138	52.319856	65.665242
1504.719458	57.419662	65.670247
1504.616285	40.194555	65.675252
1504.076518	54.967223	65.680257
1503.940611	46.364895	65.685262
1503.261519	47.507188	65.690266
1502.152435	42.099694	65.695271
1501.405372	48.153689	65.700276
1501.132210	52.587056	65.705281
1499.887273	43.214829	65.710286
1499.099302	52.913157	65.715290
1498.620342	42.011079	65.720295
1498.325491	39.583791	65.725300
1497.741026	46.381460	65.730305
1497.273184	39.126488	65.735310
1496.578447	44.156667	65.740314
1495.549511	50.860969	65.745319
1494.698006	38.914284	65.750324
1493.569666	42.922169	65.755329
1493.115270	37.662952	65.760334
1492.805119	41.053578	65.765338
1492.302069	49.922930	65.770343
1492.353291	32.808912	65.775348
1491.068307	46.987244	65.780353
1489.969562	33.512446	65.785358
1489.709601	34.736367	65.790362
1489.122075	40.019153	65.795367
1488.215182	31.977714	65.800372
1487.300424	35.860204	65.805377
1486.851482	41.612952	65.810382
1486.109532	33.835447	65.815386
1485.763170	42.455982	65.820391
1484.832084	43.791277	65.825396
1483.818292	56.855837	65.830401
1483.538421	42.330023	65.835406
1483.103392	38.813321	65.840410
1482.254745	49.964125	65.845415
1481.778112	35.004410	65.850420
1480.947947	50.439774	65.855425
1480.949740	41.176941	65.860430
1479.609349	42.012759	65.865434
1478.576897	53.612219	65.870439
1478.533644	36.874314	65.875444
1477.843480	41.943190	65.880449
1477.337453	43.611468	65.885454
1476.477489	39.064793	65.890458
1475.501477	47.115218	65.895463
1474.904203	43.050319	65.900468
1474.184393	50.238487	65.905473
1474.180396	47.884825	65.910478
1472.990017	43.731257	65.915482
1472.341578	51.412682	65.920487
1472.206273	30.155922	65.925492
1471.147532	45.671757	65.930497
1470.506807	39.196429	65.935502
1470.159796	44.511960	65.940506
1469.185883	48.208328	65.945511
1468.439705	38.911398	65.950516
1467.314784	46.129250	65.955521
1467.182325	45.393368	65.960526
1466.790775	44.968301	65.965530
1465.290586	43.595100	65.970535
1465.207874	32.035595	65.975540
1464.407741	44.940047	65.980545
1463.787246	45.098534	65.985550
1463.772373	36.882239	65.990554
1462.397728	41.459103	65.995559
1461.946856	34.739157	66.000564
1461.298332	44.491017	66.005569
1460.469775	42.777715	66.010574
1459.673704	42.741766	66.015578
1458.689732	42.551184	66.020583
1458.771983	37.987244	66.025588
1457.930678	38.234435	66.030593
1457.675785	45.523756	66.035598
1456.202272	43.600727	66.040602
1455.601475	54.928184	66.045607
1455.415059	40.390682	66.050612
1454.874824	43.122477	66.055617
1453.768702	40.639623	66.060622
1453.306253	26.059275	66.065626
1452.356417	48.685237	66.070631
1452.550739	41.869067	66.075636
1451.224611	41.986736	66.080641
1450.576728	42.152733	66.085646
1449.958983	38.237744	66.090650
1449.329907	38.463827	66.095655
1448.611358	32.768810	66.100660
1447.320175	47.017524	66.105665
1447.125728	40.941188	66.110670
1446.657011	46.443211	66.115674
1446.057687	44.430147	66.120679
1445.697370	41.453483	66.125684
1444.699469	47.623042	66.130689
1443.893110	42.832906	66.135694
1443.387457	47.844086	66.140698
1442.724759	47.551994	66.145703
1441.825209	35.669738	66.150708
1441.165082	59.418135	66.155713
1441.056509	46.109256	66.160718
1440.702613	46.454027	66.165722
1439.374948	48.451570	66.170727
1438.462966	49.853228	66.175732
1438.004491	46.084807	66.180737
1437.445944	51.224237	66.185742
1436.778334	42.283819	66.190746
1435.652492	55.005093	66.195751
1435.561958	50.981091	66.200756
1434.953584	44.137952	66.205761
1434.017288	53.260656	66.210766
1433.158055	49.253166	66.215770
1432.546651	49.500098	66.220775
1432.176312	37.562126	66.225780
1431.837815	60.526169	66.230785
1431.266993	45.209289	66.235790
1430.119920	28.116998	66.240794
1429.277870	62.642217	66.245799
1429.132830	43.173588	66.250804
1427.579040	44.828626	66.255809
1426.890428	45.444201	66.260814
1426.750492	46.787817	66.265818
1426.238105	54.029760	66.270823
1426.053112	32.433996	66.275828
1425.410570	50.124426	66.280833
1424.644104	50.829641	66.285838
1423.809895	32.572783	66.290842
1422.329519	57.722487	66.295847
1421.998701	33.719946	66.300852
1421.444422	36.211140	66.305857
1420.984766	42.383468	66.310862
1421.085711	41.725606	66.315866
1419.521307	37.262523	66.320871
1419.160431	42.061472	66.325876
1418.172371	53.461516	66.330881
1416.921759	41.406415	66.335886
1416.600691	42.980658	66.340890
1415.919151	47.232939	66.345895
1415.380849	43.545016	66.350900
1415.124673	47.931534	66.355905
1414.815986	45.642066	66.360910
1413.823590	44.424724	66.365914
1412.999487	39.493926	66.370919
1412.302743	37.650888	66.375924
1411.886367	43.434738	66.380929
1410.786880	43.204188	66.385934
1410.387693	48.387676	66.390938
1409.496989	46.376779	66.395943
1409.448819	32.165813	66.400948
1408.338560	45.184214	66.405953
1407.548302	41.755521	66.410958
1407.237450	34.705847	66.415962
1406.229790	42.430178	66.420967
1405.362717	34.432905	66.425972
1404.555693	44.025470	66.430977
1403.918056	38.921546	66.435982
1403.896335	31.788076	66.440986
1403.478276	32.715451	66.445991
1402.923332	38.187027	66.450996
1401.487829	45.928900	66.456001
1400.833763	43.405760	66.461006
1400.797455	42.246192	66.466010
1400.111664	46.232662	66.471015
1399.141213	42.321707	66.476020
1398.638143	45.525395	66.481025
1397.648653	47.522825	66.486030
1396.502180	46.074526	66.491034
1395.611152	47.791394	66.496039
1395.514844	47.593788	66.501044
1394.933898	46.605933	66.506049
1394.724326	44.950384	66.511054
1394.453298	42.740084	66.516058
1393.540353	45.427054	66.521063
1392.973828	48.035313	66.526068
1392.124216	47.824979	66.531073
1391.048011	42.950025	66.536078
1390.619460	39.982638	66.541082
1389.744990	46.443238	66.546087
1389.594858	37.239254	66.551092
1388.398215	47.395193	66.556097
1387.444426	49.377492	66.561102
1387.359315	47.110836	66.566106
1386.557119	62.571743	66.571111
1385.928924	31.501665	66.576116
1384.767999	35.970484	66.581121
1384.180230	46.628858	66.586126
1384.070285	41.674443	66.591130
1383.446626	50.269679	66.596135
1383.227008	52.696654	66.601140
1382.089574	55.100783	66.606145
1381.429251	49.171036	66.611150
1380.907068	46.694745	66.616154
1380.003779	54.115511	66.621159
1379.368963	39.326041	66.626164
1378.891156	35.992770	66.631169
1377.561632	47.901230	66.636174
1377.051536	46.361253	66.641178
1376.144477	44.024980	66.646183
1376.166693	45.377517	66.651188
1375.754119	49.905584	66.656193
1374.582241	42.565436	66.661198
1373.869097	35.472483	66.666202
1373.012811	50.513069	66.671207
1372.969523	46.915200	66.676212
1371.950500	51.761998	66.681217
1371.025001	48.264931	66.686222
1370.256600	47.393604	66.691226
1370.039393	52.401524	66.696231
1369.914057	36.671690	66.701236
1369.244191	52.111554	66.706241
1367.978454	54.961836	66.711246
1367.606005	50.828115	66.716250
1367.077167	43.008891	66.721255
1365.874928	46.430942	66.726260
1365.086467	48.088943	66.731265
1364.504759	53.410252	66.736270
1364.416951	42.226858	66.741274
1363.488559	54.353828	66.746279
1362.370543	49.286846	66.751284
1361.753875	44.335709	66.756289
1361.649460	38.472145	66.761294
1361.253314	42.360547	66.766298
1360.031515	44.486374	66.771303
1359.647417	40.050175	66.776308
1358.576999	47.875956	66.781313
1358.262718	44.950332	66.786318
1358.101057	47.686622	66.791322
1356.437917	50.022943	66.796327
1356.095186	44.939961	66.801332
1355.673500	34.216476	66.806337
1354.739802	41.446545	66.811342
1353.926340	38.909334	66.816346
1353.089486	42.057281	66.821351
1352.895550	41.611859	66.826356
1352.285268	49.993673	66.831361
1351.618755	44.977926	66.836366
1351.195837	36.761850	66.841370
1350.156663	41.375325	66.846375
1350.014735	39.652262	66.851380
1349.071021	45.991423	66.856385
1347.825670	49.238996	66.861390
1347.625979	40.161159	66.866394
1346.990544	40.801415	66.871399
1346.448512	45.651243	66.876404
1345.535070	38.407221	66.881409
1344.740598	55.547834	66.886414
1344.579486	29.570927	66.891418
1343.398481	39.561974	66.896423
1342.867059	45.720489	66.901428
1342.258905	34.823232	66.906433
1341.688465	36.856567	66.911438
1341.352613	38.149331	66.916442
1340.072057	44.614573	66.921447
1339.326743	43.749047	66.926452
1339.256237	45.441156	66.931457
1338.372053	50.985581	66.936462
1338.457361	39.205427	66.941466
1337.176538	44.256267	66.946471
1336.474620	43.388574	66.951476
1335.555456	36.851901	66.956481
1334.618480	46.772628	66.961486
1334.260633	38.632940	66.966490
1333.469623	44.424312	66.971495
1333.322208	37.400708	66.976500
1332.651108	45.672348	66.981505
1331.398399	43.550300	66.986510
1331.110173	42.164289	66.991514
1330.418242	64.654681	66.996519
1330.089150	45.204295	67.001524
1328.889646	51.787541	67.006529
1328.232979	44.425439	67.011534
1327.782072	39.663994	67.016538
1327.531833	40.255639	67.021543
1326.697611	44.615784	67.026548
1325.915196	38.069991	67.031553
1325.165215	43.769693	67.036558
1324.468689	37.304860	67.041562
1323.067004	51.452922	67.046567
1322.793014	40.303863	67.051572
1322.533965	33.178166	67.056577
1321.772340	45.389009	67.061582
1321.784324	38.671208	67.066586
1320.641526	45.623887	67.071591
1320.147590	41.616716	67.076596
1319.587265	47.062357	67.081601
1317.979000	45.070949	67.086606
1317.551877	35.944124	67.091610
1316.953151	49.989774	67.096615
1316.517598	33.801518	67.101620
1315.914863	44.008140	67.106625
1315.311180	42.017880	67.111630
1314.718232	30.585239	67.116634
1313.933481	42.560074	67.121639
1313.509472	36.793050	67.126644
1312.659043	44.757328	67.131649
1311.700518	39.824284	67.136654
1311.337063	42.132210	67.141658
1310.913184	46.099140	67.146663
1310.016574	34.166022	67.151668
1308.895200	42.901883	67.156673
1308.015496	50.009852	67.161678
1307.874153	40.027088	67.166682
1307.486164	37.986773	67.171687
1306.912814	40.307567	67.176692
1305.740882	41.373722	67.181697
1305.243672	39.927902	67.186702
1305.195601	35.551831	67.191706
1303.750139	43.170759	67.196711
1303.025308	31.402716	67.201716
1302.536604	44.979889	67.206721
1302.027545	45.387190	67.211726
1301.998083	28.934127	67.216730
1300.680485	33.181895	67.221735
1299.993145	45.841376	67.226740
1299.525189	42.877117	67.231745
1298.294728	52.131771	67.236750
1297.683233	39.776459	67.241754
1296.630784	48.993351	67.246759
1296.623628	48.956608	67.251764
1296.529461	46.238838	67.256769
1295.867651	43.803687	67.261774
1295.339779	36.179866	67.266778
1294.488046	49.387426	67.271783
1294.019731	42.034815	67.276788
1292.341135	53.456365	67.281793
1291.543339	45.096481	67.286798
1291.133219	33.887079	67.291802
1290.638934	51.643830	67.296807
1290.701112	38.916510	67.301812
1289.639286	35.765985	67.306817
1288.594792	43.557705	67.311822
1288.769966	41.859923	67.316826
1287.115653	50.677367	67.321831
1286.574838	36.680348	67.326836
1285.850765	38.777540	67.331841
1285.202650	36.124185	67.336846
1284.980767	50.895206	67.341850
1284.563722	52.686560	67.346855
1283.589802	37.903735	67.351860
1282.893802	42.737051	67.356865
1282.022560	42.232165	67.361870
1281.922709	40.084548	67.366874
1280.601557	45.666920	67.371879
1279.993453	40.071087	67.376884
1279.814279	49.024579	67.381889
1278.820341	45.409127	67.386894
1278.025505	41.979630	67.391898
1277.363387	48.203086	67.396903
1277.006302	45.952869	67.401908
1276.652119	43.647002	67.406913
1275.458664	42.382837	67.411918
1274.939158	45.135021	67.416922
1274.143291	47.019716	67.421927
1273.961159	43.112787	67.426932
1273.095298	30.820007	67.431937
1271.968289	36.768883	67.436942
1271.688684	48.540425	67.441946
1271.180578	47.055345	67.446951
1270.458399	47.644760	67.451956
1269.525432	44.095308	67.456961
1268.548969	40.144365	67.461966
1268.620504	41.116919	67.466970
1268.062119	41.457956	67.471975
1266.933097	43.081823	67.476980
1266.512514	53.415608	67.481985
1265.738920	42.699208	67.486990
1264.973484	37.601453	67.491994
1264.076764	54.797752	67.496999
1263.140012	45.893877	67.502004
1262.954700	44.967724	67.507009
1262.405948	45.622604	67.512014
1262.313301	36.918827	67.517018
1261.319143	49.321185	67.522023
1260.626294	42.732792	67.527028
1260.142154	35.363788	67.532033
1258.909666	50.076296	67.537038
1258.343695	35.323240	67.542042
1257.501418	46.320118	67.547047
1257.043796	45.888243	67.552052
1256.544847	50.441095	67.557057
1255.210432	46.119737	67.562062
1254.969773	40.451299	67.567066
1254.460793	41.623375	67.572071
1253.798489	48.917554	67.577076
1253.659940	44.084387	67.582081
1252.349584	38.056197	67.587086
1251.800190	42.844135	67.592090
1251.283855	42.784275	67.597095
1250.523320	46.494096	67.602100
1249.702281	42.114773	67.607105
1249.058466	53.034375	67.612110
1248.937472	35.862626	67.617114
1248.118339	45.960169	67.622119
1247.028930	35.525793	67.627124
1246.243959	40.354340	67.632129
1245.903376	47.305649	67.637134
1245.492432	41.271648	67.642138
1244.598919	48.220989	67.647143
1244.081953	45.439566	67.652148
1243.886526	38.190231	67.657153
1242.535849	48.160991	67.662158
1241.810172	35.686670	67.667162
1241.409702	42.305320	67.672167
1240.503430	34.546148	67.677172
1239.422891	41.126278	67.682177
1238.991837	48.240197	67.687182
1238.647913	42.312229	67.692186
1238.156790	49.358434	67.697191
1237.610911	30.317862	67.702196
1236.683555	32.237664	67.707201
1235.800403	35.966982	67.712206
1235.308638	37.804913	67.717210
1234.791857	47.188951	67.722215
1233.581776	40.064677	67.727220
1233.122953	45.908908	67.732225
1232.518251	46.009749	67.737230
1232.524237	37.219335	67.742234
1231.159899	42.652485	67.747239
1230.567799	45.977583	67.752244
1229.925190	40.951768	67.757249
1229.375607	43.683512	67.762254
1228.832043	39.157584	67.767258
1228.002597	43.375078	67.772263
1227.352039	44.214876	67.777268
1226.893000	47.320133	67.782273
1226.258812	43.811497	67.787278
1225.144897	34.834896	67.792282
1224.255469	39.511333	67.797287
1224.010200	45.867203	67.802292
1223.515264	46.997630	67.807297
1222.936103	40.681316	67.812302
1222.272698	43.675574	67.817306
1221.584738	53.520472	67.822311
1221.119604	42.346637	67.827316
1220.017595	34.599675	67.832321
1219.184909	41.328049	67.837326
1218.523849	45.752148	67.842330
1218.264644	49.696060	67.847335
1217.674444	43.411463	67.852340
1216.766541	42.078269	67.857345
1215.777718	43.791823	67.862350
1215.421611	37.824801	67.867354
1215.111182	45.047266	67.872359
1214.439845	42.769762	67.877364
1213.498457	42.641885	67.882369
1212.409262	52.124831	67.887374
1212.555346	36.741359	67.892378
1211.627321	43.645735	67.897383
1210.755798	44.866004	67.902388
1210.202750	44.909755	67.907393
1209.728950	38.869989	67.912398
1209.185922	38.606236	67.917402
1207.905496	44.243662	67.922407
1207.380566	40.728697	67.927412
1206.834316	34.828180	67.932417
1206.521357	44.053661	67.937422
1205.808738	30.050882	67.942426
1204.857063	32.591114	67.947431
1204.699653	37.827632	67.952436
1203.764164	37.534827	67.957441
1202.769715	37.383854	67.962446
1202.280350	40.099720	67.967450
1202.074448	32.088860	67.972455
1200.886788	39.747262	67.977460
1200.497744	37.284535	67.982465
1199.859821	40.238477	67.987470
1199.338691	27.914572	67.992474
1198.095219	33.449933	67.997479
1196.881981	40.890067	68.002484
1196.887265	37.498941	68.007489
1196.501784	43.902336	68.012494
1196.009806	43.177909	68.017498
1194.944701	35.570162	68.022503
1193.937537	40.533396	68.027508
1193.637884	30.260459	68.032513
1193.405148	43.104691	68.037518
1192.280446	31.054947	68.042522
1191.737723	46.537678	68.047527
1191.166035	33.436533	68.052532
1190.588427	39.220811	68.057537
1189.583743	49.765743	68.062542
1188.908601	42.912799	68.067546
1187.998003	49.046482	68.072551
1187.774885	42.377112	68.077556
1187.512852	32.110808	68.082561
1186.481596	45.785299	68.087566
1185.880950	38.192003	68.092570
1185.208377	47.294909	68.097575
1184.065372	46.355482	68.102580
1183.260350	38.747380	68.107585
1182.725253	51.400017	68.112590
1182.530009	33.478469	68.117594
1182.125373	44.189739	68.122599
1181.404190	48.309612	68.127604
1180.683766	30.848451	68.132609
1179.377897	43.847563	68.137614
1179.000143	41.712607	68.142618
1178.485863	47.004301	68.147623
1178.006195	39.494265	68.152628
1177.166935	41.081553	68.157633
1176.523194	54.872618	68.162638
1176.432901	33.405366	68.167642
1175.388764	39.470403	68.172647
1174.414759	39.618947	68.177652
1173.994087	26.973165	68.182657
1173.147853	44.118862	68.187662
1172.178908	32.290350	68.192666
1171.699094	41.138688	68.197671
1171.167825	38.148258	68.202676
1170.822691	28.737219	68.207681
1169.788817	39.753540	68.212686
1169.167837	40.166050	68.217690
1168.785198	25.658258	68.222695
1167.865558	43.835857	68.227700
1167.787326	31.972930	68.232705
1166.625689	36.568099	68.237710
1165.899496	37.255945	68.242714
1165.574675	30.530222	68.247719
1164.338127	35.944656	68.252724
1163.678181	40.316552	68.257729
1162.842280	41.282028	68.262734
1162.760282	34.511381	68.267738
1162.179549	30.965882	68.272743
1161.738052	31.351428	68.277748
1161.068970	29.767401	68.282753
1160.018752	35.314622	68.287758
1159.681163	34.950404	68.292762
1158.434814	36.715970	68.297767
1157.635070	38.680157	68.302772
1157.460115	38.996510	68.307777
1156.886810	40.951494	68.312782
1156.194313	34.009868	68.317786
1155.347333	33.252024	68.322791
1154.511520	39.115215	68.327796
1154.044009	47.371855	68.332801
1153.662952	35.486126	68.337806
1152.709032	36.397838	68.342810
1151.825229	39.449237	68.347815
1151.194214	37.851273	68.352820
1151.126149	35.988753	68.357825
1149.757128	44.161692	68.362830
1149.275090	38.537966	68.367834
1149.022358	37.203101	68.372839
1147.996487	39.436628	68.377844
1147.578250	46.756662	68.382849
1146.625931	34.780445	68.387854
1146.407749	31.882150	68.392858
1145.880122	26.617319	68.397863
1144.403324	40.889343	68.402868
1143.860209	37.430899	68.407873
1143.057074	40.327555	68.412878
1142.720199	40.802115	68.417882
1142.653217	34.208844	68.422887
1141.568328	31.199241	68.427892
1140.831465	38.346030	68.432897
1140.297835	37.875805	68.437902
1139.988958	36.187192	68.442906
1138.446973	29.202488	68.447911
1137.617612	44.019641	68.452916
1137.880312	33.252028	68.457921
1137.131952	42.988274	68.462926
1137.028406	32.979034	68.467930
1135.507368	45.077305	68.472935
1134.877935	34.383768	68.477940
1134.739635	40.503442	68.482945
1133.020951	41.907350	68.487950
1132.247463	37.127871	68.492954
1132.203521	30.925154	68.497959
1131.911823	37.908111	68.502964
1131.473556	30.451429	68.507969
1130.196387	40.915134	68.512974
1129.556652	42.153757	68.517978
1129.253075	39.901364	68.522983
1128.100176	45.368741	68.527988
1127.337466	44.113408	68.532993
1126.577204	35.441715	68.537998
1126.194921	31.721171	68.543002
1125.621354	35.508512	68.548007
1125.423114	38.353121	68.553012
1124.505719	22.607410	68.558017
1123.383406	52.372476	68.563022
1123.467980	37.806149	68.568026
1122.367124	40.644510	68.573031
1121.214372	41.024917	68.578036
1120.902281	41.795142	68.583041
1120.275068	47.651975	68.588046
1119.927661	32.596149	68.593050
1119.278466	42.048560	68.598055
1118.275960	37.694994	68.603060
1117.881569	35.639962	68.608065
1117.382934	38.619075	68.613070
1116.229188	41.806452	68.618074
1115.691739	31.790536	68.623079
1114.870702	38.534427	68.628084
1115.004998	37.771909	68.633089
1113.905102	36.783084	68.638094
1113.001379	40.678129	68.643098
1112.427010	45.763358	68.648103
1111.767542	43.595953	68.653108
1111.501977	25.286674	68.658113
1110.310918	42.988663	68.663118
1109.843630	38.751814	68.668122
1109.717686	26.805031	68.673127
1108.206665	39.658609	68.678132
1107.495227	35.170451	68.683137
1106.841323	41.323248	68.688142
1106.525471	31.746725	68.693146
1106.164984	34.705444	68.698151
1105.221939	37.591247	68.703156
1104.897380	33.784259	68.708161
1103.923890	33.910672	68.713166
1103.097956	27.133785	68.718170
1102.304015	28.838460	68.723175
1101.520784	29.180603	68.728180
1101.311335	30.491135	68.733185
1100.794675	37.968740	68.738190
1099.828710	33.544721	68.743194
1099.112034	40.773459	68.748199
1098.222511	42.490185	68.753204
1098.387545	29.174137	68.758209
1097.236965	53.185020	68.763214
1096.430118	36.738945	68.768218
1096.026853	24.703818	68.773223
1095.099507	53.427114	68.778228
1095.131499	29.373312	68.783233
1094.051806	34.535760	68.788238
1093.547561	17.052889	68.793242
1092.753084	33.271046	68.798247
1091.638036	34.465436	68.803252
1090.996730	35.879348	68.808257
1090.170342	44.763896	68.813262
1089.734519	31.951822	68.818266
1089.795937	37.587170	68.823271
1088.938820	33.622054	68.828276
1088.411366	31.526694	68.833281
1087.714358	35.660086	68.838286
1086.589012	35.189377	68.843290
1085.571554	37.759037	68.848295
1084.809288	36.807980	68.853300
1084.829061	47.358717	68.858305
1084.035375	46.362198	68.863310
1083.617738	22.118169	68.868314
1083.341683	20.407000	68.873319
1081.950703	41.207779	68.878324
1081.683665	34.505995	68.883329
1080.546881	34.109643	68.888334
1079.807716	26.669299	68.893338
1079.203266	28.646597	68.898343
1078.500602	35.849455	68.903348
1078.201172	32.437420	68.908353
1077.661923	37.755172	68.913358
1076.690926	31.300970	68.918362
1076.246452	37.850942	68.923367
1075.217655	24.917167	68.928372
1075.014220	54.309018	68.933377
1073.875704	40.530140	68.938382
1072.984233	31.830458	68.943386
1072.667547	26.732356	68.948391
1072.154491	41.906034	68.953396
1072.343271	35.268934	68.958401
1071.000846	20.420287	68.963406
1070.117298	48.017039	68.968410
1070.071213	34.573730	68.973415
1068.371699	26.103502	68.978420
1067.721501	51.676304	68.983425
1067.120592	27.947097	68.988430
1067.158251	41.716502	68.993434
1066.850603	13.661077	68.998439
1065.893972	36.303915	69.003444
1065.475065	9.119278	69.008449
1064.327699	47.857481	69.013454
1063.430377	15.937934	69.018458
1062.580995	43.822539	69.023463
1062.171951	6.659557	69.028468
1061.837910	52.648083	69.033473
1060.651788	25.150242	69.038478
1059.880250	39.694870	69.043482
1059.653378	30.988822	69.048487
1058.795995	43.183400	69.053492
1058.741426	30.843670	69.058497
1057.848099	31.912925	69.063502
1056.988686	25.541904	69.068506
1056.491886	41.545578	69.073511
1055.883031	43.544082	69.078516
1054.980076	23.958036	69.083521
1054.096097	37.509784	69.088526
1053.703752	41.298273	69.093530
1053.530828	38.118415	69.098535
1052.073170	11.890594	69.103540
1051.470208	39.024831	69.108545
1050.878771	33.230888	69.113550
1050.646727	33.004428	69.118554
1049.439288	18.151671	69.123559
1048.385506	68.132219	69.128564
1048.173750	19.846192	69.133569
1047.732371	55.878187	69.138574
1047.701364	31.977908	69.143578
1046.587089	41.217323	69.148583
1045.707196	41.852386	69.153588
1045.488252	26.739886	69.158593
1044.218607	34.433463	69.163598
1043.242501	41.031739	69.168602
1043.018324	33.235112	69.173607
1042.620792	33.793446	69.178612
1042.380479	25.696633	69.183617
1041.102896	42.986652	69.188622
1040.393506	25.405546	69.193626
1040.103981	51.662096	69.198631
1038.972758	22.944515	69.203636
1038.171378	38.957215	69.208641
1037.552579	43.773574	69.213646
1037.195197	15.696110	69.218650
1036.855475	45.007118	69.223655
1035.816090	35.574088	69.228660
1034.830443	28.876247	69.233665
1034.293409	37.282716	69.238670
1033.855226	24.608227	69.243674
1033.306759	44.773563	69.248679
1032.381371	39.606723	69.253684
1031.650634	32.786336	69.258689
1031.244274	36.870351	69.263694
1030.980909	42.697702	69.268698
1030.148001	45.299523	69.273703
1029.204860	44.791971	69.278708
1028.732364	17.313103	69.283713
1028.092938	46.022123	69.288718
1026.684718	26.967447	69.293722
1026.042297	43.524112	69.298727
1025.395281	45.393085	69.303732
1025.289335	28.638448	69.308737
1024.991655	48.117382	69.313742
1024.570606	16.333396	69.318746
1023.333351	43.913874	69.323751
1022.737843	30.244184	69.328756
1022.428089	50.702693	69.333761
1021.434090	17.212233	69.338766
1020.591909	51.275404	69.343770
1020.673580	31.742454	69.348775
1018.964883	40.593921	69.353780
1018.464825	40.085267	69.358785
1017.878008	37.406468	69.363790
1017.319545	13.422991	69.368794
1016.883725	38.701484	69.373799
1015.802709	29.476930	69.378804
1015.558085	33.552562	69.383809
1014.652823	47.563424	69.388814
1014.415932	33.740496	69.393818
1013.207268	33.604754	69.398823
1012.209867	49.911988	69.403828
1011.953875	32.869001	69.408833
1011.432874	32.581288	69.413838
1011.004905	36.093191	69.418842
1010.166041	41.099095	69.423847
1009.573494	50.250798	69.428852
1009.394322	27.548868	69.433857
1007.934660	34.771249	69.438862
1007.100571	47.416269	69.443866
1006.561529	19.438670	69.448871
1006.227762	44.166382	69.453876
1005.642713	16.002156	69.458881
1004.620740	42.406744	69.463886
1004.259018	37.743143	69.468890
1003.686596	15.821265	69.473895
1002.592955	49.389881	69.478900
1002.119563	32.692124	69.483905
1001.211631	24.903368	69.488910
1000.747041	56.113868	69.493914
1000.790595	21.329319	69.498919
999.133047	57.591055	69.503924
998.985004	16.201579	69.508929
998.209331	53.614451	69.513934
997.742635	38.547673	69.518938
996.967454	27.596699	69.523943
996.255867	55.759008	69.528948
995.300260	29.957504	69.533953
994.859222	53.965906	69.538958
993.754202	30.037828	69.543962
993.363044	52.701118	69.548967
992.565156	16.814193	69.553972
992.360686	42.377562	69.558977
992.362415	14.676624	69.563982
990.972175	49.968626	69.568986
990.383561	26.070357	69.573991
989.409413	56.258124	69.578996
989.275464	17.034590	69.584001
988.022639	62.499128	69.589006
986.472517	36.421640	69.594010
986.784849	30.431897	69.599015
986.222976	53.251648	69.604020
986.526580	28.323660	69.609025
985.516266	39.131294	69.614030
984.321627	53.386890	69.619034
984.151764	33.952305	69.624039
982.797039	27.308477	69.629044
982.141296	45.183941	69.634049
981.681157	30.781567	69.639054
980.739057	55.796879	69.644058
980.628625	18.064466	69.649063
979.654225	40.079406	69.654068
978.887414	43.817101	69.659073
978.740774	36.209985	69.664078
977.904784	33.450999	69.669082
977.464912	38.456507	69.674087
976.596279	33.835717	69.679092
975.605272	24.778205	69.684097
974.557783	36.372297	69.689102
973.729186	44.713208	69.694106
973.681799	15.367543	69.699111
973.047796	54.790441	69.704116
972.481951	35.474048	69.709121
972.242943	29.920507	69.714126
971.087733	23.569778	69.719130
970.678523	44.611764	69.724135
970.072635	43.312608	69.729140
968.755076	26.949439	69.734145
968.386252	36.902854	69.739150
967.808787	48.209301	69.744154
967.550493	18.088260	69.749159
966.400612	34.643661	69.754164
965.699289	48.108031	69.759169
965.337728	25.424099	69.764174
964.628677	34.526529	69.769178
963.656925	44.661028	69.774183
962.581406	36.406966	69.779188
962.461967	32.136886	69.784193
962.240798	44.105688	69.789198
961.262685	29.891383	69.794202
960.702620	40.851302	69.799207
959.873235	17.740378	69.804212
959.124289	13.745492	69.809217
958.629019	51.455918	69.814222
957.590420	10.201866	69.819226
956.981005	42.777274	69.824231
956.198209	44.956431	69.829236
956.063561	13.653589	69.834241
955.720152	62.444087	69.839246
954.592735	43.256464	69.844250
954.273911	17.084051	69.849255
953.286494	54.155318	69.854260
952.634283	37.208499	69.859265
951.401786	18.980589	69.864270
950.885306	40.017559	69.869274
951.005795	30.869934	69.874279
950.317686	39.270490	69.879284
949.752825	36.540910	69.884289
948.451815	38.687411	69.889294
947.971041	42.740703	69.894298
947.341399	23.172730	69.899303
946.140105	44.921026	69.904308
945.608699	40.375892	69.909313
945.283610	31.765912	69.914318
944.599423	24.993343	69.919322
944.668780	35.189256	69.924327
943.192682	36.207782	69.929332
942.713289	25.211345	69.934337
942.033990	28.982428	69.939342
941.728944	48.137694	69.944346
940.910243	28.181932	69.949351
939.764938	35.668123	69.954356
939.549590	28.977064	69.959361
938.932935	44.820052	69.964366
937.873122	37.795028	69.969370
937.505701	26.580516	69.974375
936.744139	29.524226	69.979380
936.300053	20.710852	69.984385
935.564254	29.144223	69.989390
934.449499	39.870725	69.994394
934.283983	31.881868	69.999399
933.837463	34.806989	70.004404
933.043342	35.179300	70.009409
932.251198	27.618138	70.014414
931.653392	53.898496	70.019418
931.254375	33.085948	70.024423
929.862050	46.497855	70.029428
929.513151	27.036593	70.034433
928.896787	26.429777	70.039438
927.765963	25.728214	70.044442
927.105731	48.945207	70.049447
926.387132	41.282457	70.054452
926.182546	33.774451	70.059457
925.635452	25.915696	70.064462
925.009942	39.194546	70.069466
924.948213	39.032455	70.074471
923.753040	29.547011	70.079476
923.097276	41.075637	70.084481
922.110182	26.681448	70.089486
920.995601	30.509183	70.094490
920.790820	22.072447	70.099495
920.031928	42.747472	70.104500
920.175708	19.289341	70.109505
918.775193	29.208233	70.114510
918.064290	30.972284	70.119514
917.675383	20.248449	70.124519
917.122407	38.044481	70.129524
916.596966	32.668982	70.134529
915.833396	31.413853	70.139534
914.752731	27.821824	70.144538
914.581620	27.109471	70.149543
913.395782	33.909881	70.154548
912.738072	40.425997	70.159553
912.452207	40.502986	70.164558
911.972060	46.270227	70.169562
910.973972	26.402949	70.174567
910.317830	42.923960	70.179572
909.478892	21.777765	70.184577
909.349611	34.965035	70.189582
908.074521	30.565059	70.194586
907.635945	22.819923	70.199591
906.741953	41.226853	70.204596
906.532397	30.168564	70.209601
905.827782	37.337077	70.214606
904.655643	40.183715	70.219610
904.658389	28.265372	70.224615
903.615636	32.267754	70.229620
903.350150	30.548618	70.234625
902.301316	31.418758	70.239630
901.647967	30.789451	70.244634
901.548069	23.573859	70.249639
900.494419	34.233877	70.254644
899.854739	34.540624	70.259649
898.950272	35.518671	70.264654
898.231009	37.742924	70.269658
898.189215	37.681734	70.274663
896.719379	34.919568	70.279668
896.006050	28.788701	70.284673
895.508198	33.655219	70.289678
895.041693	49.128989	70.294682
895.158460	22.679130	70.299687
893.928160	36.530431	70.304692
892.990607	37.015459	70.309697
892.873386	36.278764	70.314702
892.207030	41.211520	70.319706
891.502692	33.855582	70.324711
890.589479	37.044197	70.329716
889.846835	35.205464	70.334721
888.846158	36.197248	70.339726
888.258886	39.999430	70.344730
888.269174	29.014964	70.349735
887.564577	35.680461	70.354740
886.923875	35.772921	70.359745
886.024484	29.808852	70.364750
885.222558	33.157944	70.369754
884.816095	34.346888	70.374759
883.542937	29.840969	70.379764
883.087045	34.238793	70.384769
882.530492	31.706593	70.389774
882.017956	37.882663	70.394778
881.665963	23.918831	70.399783
880.701126	33.735297	70.404788
880.106155	28.244726	70.409793
879.323655	30.641461	70.414798
877.816040	34.135970	70.419802
877.827181	27.421494	70.424807
877.064495	34.425798	70.429812
876.845596	29.559735	70.434817
876.612875	26.480871	70.439822
874.933577	32.445249	70.444826
874.277248	24.170260	70.449831
873.970983	36.740760	70.454836
873.310853	18.164792	70.459841
873.173167	35.484751	70.464846
872.109534	36.264224	70.469850
871.401899	30.354795	70.474855
870.417552	33.999410	70.479860
870.070155	32.275968	70.484865
869.162622	28.929203	70.489870
868.137345	40.234384	70.494874
868.261387	29.304352	70.499879
867.544627	30.454376	70.504884
867.135206	33.733125	70.509889
866.321256	20.864619	70.514894
865.560755	28.980257	70.519898
865.088485	25.534266	70.524903
863.797392	32.416097	70.529908
862.801048	27.751027	70.534913
862.487514	32.216078	70.539918
861.943189	37.854772	70.544922
861.992427	29.030710	70.549927
860.800174	32.028790	70.554932
860.010582	28.038826	70.559937
859.998079	37.372601	70.564942
858.829973	33.471258	70.569946
858.380366	32.178796	70.574951
857.492257	29.180583	70.579956
857.055256	27.949190	70.584961
856.312096	23.463014	70.589966
854.938121	34.325402	70.594970
854.648562	38.949057	70.599975
854.203209	38.028056	70.604980
853.873084	31.205475	70.609985
853.208228	36.625247	70.614990
851.703815	36.940324	70.619994
851.495154	29.601704	70.624999
851.189560	48.645093	70.630004
850.203405	47.836966	70.635009
849.722562	37.071002	70.640014
849.288096	27.712103	70.645018
848.578584	31.623625	70.650023
847.278516	39.984407	70.655028
846.667054	36.223123	70.660033
846.223536	24.530346	70.665038
845.783142	34.673338	70.670042
845.586946	28.851246	70.675047
844.328838	39.788237	70.680052
843.822007	25.180472	70.685057
843.065387	28.224339	70.690062
842.016735	45.585215	70.695066
841.255251	36.861794	70.700071
840.892289	28.560623	70.705076
840.413749	23.623933	70.710081
839.886320	37.158398	70.715086
838.503965	30.075958	70.720090
838.247882	31.602075	70.725095
837.693933	26.021415	70.730100
837.404739	38.177640	70.735105
836.590989	30.221010	70.740110
835.872275	30.877798	70.745114
835.197517	31.045073	70.750119
834.158961	33.818444	70.755124
833.343697	33.128198	70.760129
833.032661	32.058099	70.765134
832.127369	35.576612	70.770138
832.273461	31.347857	70.775143
831.175419	35.322798	70.780148
830.280073	33.675533	70.785153
829.941100	29.229108	70.790158
829.263479	33.778915	70.795162
828.639669	23.521393	70.800167
827.712805	20.231336	70.805172
827.013493	25.539907	70.810177
826.633867	18.452420	70.815182
825.203213	33.482000	70.820186
824.988141	31.595588	70.825191
824.268638	34.158920	70.830196
824.187521	33.172070	70.835201
823.533711	25.161609	70.840206
822.331206	28.142415	70.845210
821.752958	24.265475	70.850215
821.271828	30.151141	70.855220
820.557057	29.279335	70.860225
819.547156	22.162862	70.865230
818.792389	41.135811	70.870234
818.442660	24.613980	70.875239
818.164461	25.732059	70.880244
817.258710	28.861166	70.885249
816.554312	34.542689	70.890254
815.722031	31.381074	70.895258
815.774076	31.252914	70.900263
814.532718	27.729083	70.905268
813.494414	29.124252	70.910273
813.073783	26.160454	70.915278
812.505658	32.949314	70.920282
812.653189	20.331476	70.925287
811.413819	33.605540	70.930292
810.567398	38.327291	70.935297
810.463861	19.435694	70.940302
808.678156	27.878512	70.945306
808.324946	35.203987	70.950311
807.530696	32.558261	70.955316
807.228856	32.467504	70.960321
807.038016	27.264269	70.965326
806.380621	22.341864	70.970330
805.291260	20.894213	70.975335
804.531644	37.449041	70.980340
804.077298	25.079953	70.985345
803.679647	28.107693	70.990350
802.539976	28.801532	70.995354
802.237247	20.192763	71.000359
801.782403	23.414097	71.005364
800.440976	29.644841	71.010369
799.976584	23.871754	71.015374
799.427420	31.660475	71.020378
799.059693	30.134232	71.025383
798.103108	36.360493	71.030388
797.240170	40.291720	71.035393
796.852786	32.735566	71.040398
796.085119	34.384113	71.045402
795.310635	29.075094	71.050407
794.427807	32.288864	71.055412
794.084390	32.242572	71.060417
793.840136	24.001363	71.065422
792.588271	29.290666	71.070426
791.927709	24.332501	71.075431
791.612048	30.414169	71.080436
790.807973	31.686914	71.085441
790.178968	34.513377	71.090446
789.207680	33.466382	71.095450
789.012404	23.907013	71.100455
788.502501	40.210800	71.105460
787.296710	28.879053	71.110465
786.243366	26.203617	71.115470
785.562964	37.767717	71.120474
785.413956	29.751028	71.125479
785.365963	40.369274	71.130484
784.545224	32.363317	71.135489
783.890100	26.636361	71.140494
782.746656	32.062944	71.145498
782.812850	30.238991	71.150503
781.605526	28.717093	71.155508
780.752680	27.398952	71.160513
780.269399	18.233917	71.165518
779.373946	35.784861	71.170522
778.371087	23.406905	71.175527
777.818309	26.922935	71.180532
777.291862	30.068944	71.185537
777.096233	32.186224	71.190542
776.666755	39.093362	71.195546
776.023284	30.589290	71.200551
774.988882	24.049134	71.205556
774.227948	24.329485	71.210561
774.039065	27.347649	71.215566
772.618969	28.450392	71.220570
772.206893	26.303627	71.225575
771.609333	26.077033	71.230580
770.994794	25.643421	71.235585
770.173476	17.412080	71.240590
769.310042	24.834539	71.245594
768.867186	21.174167	71.250599
768.408912	26.054899	71.255604
767.844449	31.282099	71.260609
766.851302	22.843158	71.265614
765.984485	26.779739	71.270618
765.612330	28.395296	71.275623
765.396339	20.635265	71.280628
764.618393	29.482207	71.285633
763.895319	29.296093	71.290638
763.010210	35.041084	71.295642
762.490116	26.178357	71.300647
761.370909	26.028496	71.305652
760.646778	21.294912	71.310657
760.169573	25.262509	71.315662
760.194705	35.006571	71.320666
759.447823	15.356441	71.325671
758.490223	19.837295	71.330676
757.635778	27.337169	71.335681
757.146841	15.755729	71.340686
756.662661	36.484791	71.345690
755.756569	38.281534	71.350695
754.800476	29.406216	71.355700
754.649160	29.879670	71.360705
754.317308	23.577749	71.365710
753.099849	31.622661	71.370714
752.425883	23.804656	71.375719
752.029896	25.775646	71.380724
751.392963	33.475850	71.385729
750.819343	29.221324	71.390734
749.928712	31.113371	71.395738
748.828592	26.898507	71.400743
748.046282	28.918382	71.405748
747.084770	24.632572	71.410753
746.889592	27.366329	71.415758
746.421204	27.928103	71.420762
746.221279	27.978816	71.425767
745.622067	29.193733	71.430772
744.419791	30.405311	71.435777
743.946296	18.960177	71.440782
743.264422	44.184784	71.445786
742.855837	29.474685	71.450791
741.838677	25.596679	71.455796
740.964692	29.521795	71.460801
740.478153	32.920061	71.465806
739.892792	42.821232	71.470810
739.701405	29.949859	71.475815
738.531744	21.335619	71.480820
737.913989	18.595595	71.485825
737.866584	30.814239	71.490830
736.300365	35.346264	71.495834
735.515872	25.967431	71.500839
735.122166	40.608066	71.505844
734.756296	31.593067	71.510849
734.329112	17.940857	71.515854
733.101225	29.711956	71.520858
732.523670	31.536823	71.525863
732.284575	27.998552	71.530868
731.561700	36.414141	71.535873
730.717015	18.269718	71.540878
729.882372	31.835746	71.545882
729.134655	19.882373	71.550887
729.026963	27.146687	71.555892
728.114826	38.383435	71.560897
727.373983	18.497406	71.565902
726.542308	35.005368	71.570906
726.186755	40.025865	71.575911
725.735575	23.264767	71.580916
724.418358	29.756604	71.585921
724.163086	28.527841	71.590926
723.543866	30.576950	71.595930
722.732070	21.937283	71.600935
721.575262	34.813485	71.605940
720.966354	36.070950	71.610945
720.846580	11.032250	71.615950
720.183543	36.283805	71.620954
719.762910	36.234047	71.625959
718.697708	25.163796	71.630964
718.122334	32.420572	71.635969
718.228477	29.278319	71.640974
716.852527	31.045803	71.645978
715.989740	26.890936	71.650983
715.557660	36.796087	71.655988
714.941641	25.413069	71.660993
714.238377	24.006487	71.665998
713.086666	32.972866	71.671002
712.761407	27.947152	71.676007
712.509899	19.814341	71.681012
711.838823	26.444573	71.686017
711.347329	28.867562	71.691022
710.165994	33.376171	71.696026
709.221341	26.175249	71.701031
708.338313	36.715128	71.706036
707.835191	29.617365	71.711041
707.807993	19.873570	71.716046
707.208618	26.531808	71.721050
706.351111	21.876244	71.726055
705.894716	13.120088	71.731060
705.188934	24.241981	71.736065
704.708826	16.856728	71.741070
703.267776	16.247233	71.746074
702.588156	18.610292	71.751079
702.282614	26.953132	71.756084
701.853954	31.742433	71.761089
700.906977	19.510157	71.766094
699.649507	22.249049	71.771098
699.050479	24.733312	71.776103
698.846313	21.440204	71.781108
698.436202	29.000231	71.786113
698.418747	26.716541	71.791118
697.139319	31.899896	71.796122
696.620565	26.334171	71.801127
696.211333	32.572660	71.806132
694.652984	28.380316	71.811137
694.116217	19.261666	71.816142
693.515560	35.359139	71.821146
693.230346	26.511074	71.826151
692.509799	20.605344	71.831156
691.359338	25.487487	71.836161
691.084193	17.435711	71.841166
690.804723	22.109800	71.846170
689.921530	19.501930	71.851175
688.917466	19.836784	71.856180
687.864423	38.852501	71.861185
688.085055	21.427829	71.866190
687.262860	18.996316	71.871194
686.134247	40.214311	71.876199
685.464659	16.398485	71.881204
684.927918	31.982764	71.886209
684.513370	19.175326	71.891214
684.188332	37.371858	71.896218
683.446478	16.921502	71.901223
682.560238	38.752145	71.906228
681.992292	26.345992	71.911233
680.857244	21.587979	71.916238
680.067827	36.206463	71.921242
679.516174	36.155496	71.926247
679.577993	28.543621	71.931252
678.885049	24.122046	71.936257
677.771088	31.884021	71.941262
677.072468	22.501002	71.946266
676.513572	32.208738	71.951271
676.200926	25.485909	71.956276
674.584374	28.378174	71.961281
674.472862	24.215664	71.966286
673.723551	22.551515	71.971290
673.531977	38.497133	71.976295
673.063536	12.372321	71.981300
671.784479	46.976502	71.986305
671.156514	4.633959	71.991310
670.663515	39.180770	71.996314
669.869484	17.685391	72.001319
669.493232	17.269053	72.006324
668.347074	8.524970	72.011329
668.291853	27.679827	72.016334
667.302990	26.206776	72.021338
666.593555	30.826335	72.026343
666.635085	10.754280	72.031348
665.449981	9.224174	72.036353
664.602373	25.763055	72.041358
663.936416	27.463249	72.046362
663.253018	19.807619	72.051367
662.466361	31.631485	72.056372
661.431947	31.368825	72.061377
660.966463	23.043027	72.066382
660.377445	31.596576	72.071386
660.632367	11.514197	72.076391
660.181217	12.323960	72.081396
658.726553	33.064044	72.086401
658.050123	25.997045	72.091406
657.293584	20.614264	72.096410
656.343819	24.191949	72.101415
656.098871	17.387390	72.106420
655.026682	20.139376	72.111425
654.893192	18.452868	72.116430
654.496070	29.978182	72.121434
653.302213	28.299673	72.126439
652.727082	20.800260	72.131444
652.356665	27.657002	72.136449
651.507073	12.774336	72.141454
650.629580	20.430858	72.146458
649.773417	19.222095	72.151463
649.565942	21.055856	72.156468
648.822015	37.357485	72.161473
648.047173	24.003489	72.166478
647.185759	25.840459	72.171482
646.943091	21.776101	72.176487
646.574540	15.959411	72.181492
645.373266	16.987960	72.186497
644.970771	15.721154	72.191502
643.911661	28.402057	72.196506
643.589487	20.192208	72.201511
642.640240	18.194077	72.206516
641.837864	24.403710	72.211521
641.197379	14.825386	72.216526
640.721593	25.916975	72.221530
640.698740	28.123437	72.226535
640.227782	18.330472	72.231540
638.866138	18.134119	72.236545
638.703595	16.073795	72.241550
637.282331	26.037112	72.246554
636.586927	26.907849	72.251559
636.170773	24.167287	72.256564
635.617876	10.233956	72.261569
635.093711	25.565509	72.266574
633.958924	22.245565	72.271578
633.516613	22.136199	72.276583
633.227463	19.447951	72.281588
632.592533	16.319632	72.286593
631.348627	17.976255	72.291598
630.696959	27.886411	72.296602
630.521325	25.935396	72.301607
629.984021	6.918980	72.306612
629.029594	32.655290	72.311617
628.098962	18.648071	72.316622
628.250613	21.706625	72.321626
626.934384	19.503603	72.326631
626.021246	19.723085	72.331636
625.223141	18.377361	72.336641
625.056851	13.383121	72.341646
624.884866	14.552110	72.346650
623.597408	25.555344	72.351655
623.416694	16.512476	72.356660
622.662094	25.760977	72.361665
621.550582	10.774966	72.366670
620.773899	18.956301	72.371674
620.322925	23.402255	72.376679
620.078227	16.321715	72.381684
618.903343	18.434100	72.386689
618.260562	17.435780	72.391694
617.219971	23.345908	72.396698
617.005168	15.387034	72.401703
617.051719	18.531704	72.406708
615.771266	21.502938	72.411713
615.185593	16.651170	72.416718
614.470011	11.260310	72.421722
614.013277	24.464996	72.426727
613.077988	25.074337	72.431732
612.121484	19.595692	72.436737
611.917316	14.039820	72.441742
611.427424	25.688708	72.446746
610.367770	19.854353	72.451751
609.685826	9.177276	72.456756
608.790468	25.808918	72.461761
608.564852	20.686939	72.466766
607.993162	9.498751	72.471770
607.292107	26.561470	72.476775
606.871487	6.055284	72.481780
605.740669	29.156385	72.486785
605.295045	21.871314	72.491790
604.378874	15.809125	72.496794
603.477306	38.201997	72.501799
603.560516	16.633186	72.506804
602.501314	16.376076	72.511809
601.672693	35.575250	72.516814
600.846354	19.253966	72.521818
600.521589	11.427718	72.526823
600.540248	27.221573	72.531828
599.111609	16.896777	72.536833
598.136649	18.565776	72.541838
597.825603	8.463531	72.546842
597.090972	28.376232	72.551847
597.115087	17.399069	72.556852
595.731041	7.404626	72.561857
595.315126	35.328999	72.566862
594.565835	10.869954	72.571866
594.259625	35.389790	72.576871
593.719562	17.077090	72.581876
592.668993	18.658791	72.586881
592.339418	16.916787	72.591886
591.147847	21.245736	72.596890
590.165663	21.613412	72.601895
589.908970	30.323768	72.606900
589.240391	26.689920	72.611905
588.965917	10.542523	72.616910
588.005283	22.682664	72.621914
586.958465	23.580995	72.626919
586.826142	0.496495	72.631924
586.252801	26.484324	72.636929
585.778103	27.584837	72.641934
584.824893	17.411403	72.646938
583.812025	8.840092	72.651943
583.937709	14.165551	72.656948
582.288484	15.208701	72.661953
581.628554	17.026219	72.666958
581.282364	13.367840	72.671962
580.673040	11.280910	72.676967
580.774456	5.274284	72.681972
579.937652	23.506564	72.686977
579.343647	21.650566	72.691982
577.922216	15.547437	72.696986
577.077379	21.312869	72.701991
576.336969	8.218348	72.706996
575.982426	28.337005	72.712001
575.956022	12.506470	72.717006
574.844287	15.714187	72.722010
573.805407	26.938034	72.727015
573.706400	17.524216	72.732020
572.987708	31.980071	72.737025
572.533496	24.308470	72.742030
571.506505	13.847194	72.747034
571.071020	23.437517	72.752039
570.303825	23.848228	72.757044
569.202182	30.332609	72.762049
568.587951	14.800682	72.767054
568.186599	17.083189	72.772058
567.403613	20.479810	72.777063
567.021172	15.078484	72.782068
565.703877	22.798766	72.787073
565.330670	16.978104	72.792078
565.084255	24.985123	72.797082
564.515096	22.576428	72.802087
563.953587	15.981564	72.807092
562.885026	16.813986	72.812097
562.345225	15.564331	72.817102
561.671038	19.402488	72.822106
560.401315	21.711341	72.827111
559.916447	14.929242	72.832116
559.122105	22.041149	72.837121
559.047465	21.348150	72.842126
558.880650	14.810268	72.847130
558.086053	18.618721	72.852135
557.247931	27.960958	72.857140
556.275144	24.331418	72.862145
555.987329	28.503832	72.867150
554.720989	19.602340	72.872154
554.035841	27.775423	72.877159
553.634353	21.699086	72.882164
553.211146	18.937589	72.887169
552.692410	14.190289	72.892174
551.796201	25.282616	72.897178
550.994367	25.323560	72.902183
549.839191	23.150119	72.907188
548.712127	28.949474	72.912193
549.130915	22.908062	72.917198
548.406162	25.782940	72.922202
547.937362	23.080741	72.927207
547.718844	17.224407	72.932212
546.660037	25.668301	72.937217
545.790561	22.208380	72.942222
545.444973	27.642013	72.947226
544.108814	28.509179	72.952231
543.534733	12.734342	72.957236
542.684696	16.841768	72.962241
542.485852	24.341350	72.967246
542.341253	21.163345	72.972250
540.757209	29.019160	72.977255
540.462053	25.869864	72.982260
539.727779	24.748952	72.987265
539.660978	14.659851	72.992270
538.807657	12.684329	72.997274
537.648309	23.154716	73.002279
537.379199	15.075205	73.007284
536.129808	23.912130	73.012289
535.103137	9.691622	73.017294
534.995011	17.837450	73.022298
534.380039	28.326786	73.027303
534.487784	12.679883	73.032308
533.485192	18.706979	73.037313
532.784765	10.741897	73.042318
531.764707	19.827704	73.047322
531.506262	26.426939	73.052327
530.435501	7.560183	73.057332
529.267443	20.242695	73.062337
529.245754	25.643662	73.067342
528.824115	18.157686	73.072346
528.063735	12.307244	73.077351
527.329419	13.818100	73.082356
526.780390	40.327168	73.087361
526.293660	14.363021	73.092366
525.033602	29.655685	73.097370
524.212708	10.741246	73.102375
524.021107	33.194490	73.107380
523.290533	24.138297	73.112385
522.564354	9.661790	73.117390
521.369561	12.412857	73.122394
520.566965	10.186428	73.127399
520.430102	16.279048	73.132404
519.952141	33.769842	73.137409
519.918668	17.579340	73.142414
519.544034	7.950835	73.147418
518.432443	20.277452	73.152423
517.648914	28.634935	73.157428
516.215724	16.688345	73.162433
515.403514	21.679097	73.167438
515.217447	22.206982	73.172442
514.749854	11.689750	73.177447
514.299913	32.364460	73.182452
513.762163	4.883651	73.187457
512.749842	23.419845	73.192462
512.322553	20.878188	73.197466
511.496213	9.101434	73.202471
510.511927	14.769253	73.207476
510.283060	24.687769	73.212481
509.570014	7.676762	73.217486
508.783281	25.897925	73.222490
507.771899	11.020605	73.227495
507.257424	32.131342	73.232500
506.966218	19.413115	73.237505
506.408823	20.511046	73.242510
505.334635	5.911800	73.247514
504.693839	18.754745	73.252519
504.248099	17.091179	73.257524
503.517398	15.786796	73.262529
502.655086	14.224275	73.267534
502.164319	5.607688	73.272538
501.144521	29.441704	73.277543
501.501527	7.088199	73.282548
500.196900	1.516839	73.287553
499.169043	26.492193	73.292558
499.079048	-1.419439	73.297562
498.239037	32.293258	73.302567
497.404572	0.914457	73.307572
496.639609	36.789678	73.312577
496.131972	9.397107	73.317582
495.953915	22.478562	73.322586
494.729792	28.123099	73.327591
494.331331	1.709720	73.332596
493.264433	36.604934	73.337601
493.394762	1.483546	73.342606
492.238912	29.431147	73.347610
491.566202	8.148353	73.352615
491.339580	33.199503	73.357620
490.643079	17.157197	73.362625
489.527936	21.669544	73.367630
488.863159	24.128057	73.372634
488.149450	18.156660	73.377639
487.696293	43.836807	73.382644
486.693974	3.146652	73.387649
485.916878	35.311911	73.392654
485.833465	25.788391	73.397658
485.397799	31.140191	73.402663
484.604152	14.449513	73.407668
483.233152	11.102623	73.412673
483.245093	28.409722	73.417678
482.647915	9.828652	73.422682
481.273583	9.098280	73.427687
480.723799	29.634358	73.432692
479.920998	18.229152	73.437697
479.859241	30.125221	73.442702
479.327673	15.676071	73.447706
478.099540	27.627059	73.452711
477.495313	33.317928	73.457716
476.893273	9.821026	73.462721
476.729082	24.112866	73.467726
475.972653	27.513168	73.472730
475.260295	23.298166	73.477735
474.699748	12.119286	73.482740
473.768532	17.885890	73.487745
472.754459	9.955026	73.492750
471.825208	26.320875	73.497754
471.464201	24.596511	73.502759
471.275258	16.020150	73.507764
471.007856	21.576940	73.512769
469.999427	17.450103	73.517774
469.660823	5.201464	73.522778
468.391470	29.218732	73.527783
467.498137	8.459918	73.532788
466.645722	20.595463	73.537793
466.263505	22.687292	73.542798
465.853895	9.603196	73.547802
465.111260	24.234747	73.552807
464.926922	16.088132	73.557812
463.703792	18.194080	73.562817
463.196125	30.471821	73.567822
462.959364	13.039628	73.572826
461.654341	13.569162	73.577831
461.342948	19.270146	73.582836
460.610577	22.084762	73.587841
459.898937	24.298452	73.592846
459.371501	14.801526	73.597850
458.140991	28.165753	73.602855
457.541673	14.233573	73.607860
457.100575	23.025338	73.612865
456.642152	24.799748	73.617870
455.840943	17.364798	73.622874
454.892822	23.069453	73.627879
454.919281	8.514077	73.632884
454.391098	26.053859	73.637889
453.273789	28.144532	73.642894
452.829693	29.178697	73.647898
451.940443	23.339348	73.652903
451.554963	8.261434	73.657908
450.526137	13.083296	73.662913
449.468943	19.008740	73.667918
449.470604	13.688165	73.672922
448.569971	28.825831	73.677927
448.009241	19.327902	73.682932
447.107333	19.164063	73.687937
446.449879	29.325888	73.692942
446.178656	18.570821	73.697946
445.593895	22.090428	73.702951
444.637701	21.656137	73.707956
444.073417	27.424219	73.712961
443.453514	27.530824	73.717966
442.841625	27.819067	73.722970
441.625592	17.012685	73.727975
441.150777	30.152458	73.732980
440.707707	25.997061	73.737985
440.217881	22.462507	73.742990
439.564605	10.330231	73.747994
438.254066	28.187030	73.752999
438.109560	1.633878	73.758004
437.579841	38.846628	73.763009
436.922299	14.716804	73.768014
436.009037	14.622583	73.773018
435.049100	28.587065	73.778023
435.002490	17.559691	73.783028
434.410050	13.076459	73.788033
433.378156	33.835997	73.793038
432.968047	22.894913	73.798042
432.102984	13.872803	73.803047
431.589878	32.107156	73.808052
430.802269	28.933837	73.813057
429.902308	23.531413	73.818062
429.552042	24.183227	73.823066
429.112225	42.259270	73.828071
428.343812	28.500675	73.833076
427.516851	19.691675	73.838081
426.800084	18.853418	73.843086
426.778257	33.106813	73.848090
425.433441	29.175501	73.853095
425.124468	31.336087	73.858100
424.389546	33.389505	73.863105
422.821356	30.419391	73.868110
422.219397	28.123183	73.873114
421.616496	39.577225	73.878119
421.264697	26.570643	73.883124
420.892267	33.739941	73.888129
420.539398	34.676005	73.893134
420.452059	18.850470	73.898138
419.203460	19.512954	73.903143
418.700578	33.417242	73.908148
417.181084	41.759554	73.913153
416.326381	29.512716	73.918158
415.813812	16.230581	73.923162
415.457519	19.910899	73.928167
415.178667	17.116971	73.933172
414.925613	22.042317	73.938177
413.611422	31.015767	73.943182
413.247301	26.858836	73.948186
412.408257	8.169688	73.953191
411.740202	19.869045	73.958196
410.747687	32.957272	73.963201
410.028210	25.275942	73.968206
409.704978	20.767169	73.973210
409.258805	17.775987	73.978215
408.590583	17.436168	73.983220
407.687369	24.581227	73.988225
407.048532	32.693349	73.993230
406.658893	24.117433	73.998234
405.469730	19.905888	74.003239
404.882959	36.594061	74.008244
404.212771	25.718074	74.013249
403.981046	27.916812	74.018254
403.303643	24.284428	74.023258
402.384696	23.298631	74.028263
401.916023	31.036735	74.033268
401.084100	26.299949	74.038273
400.215385	36.673629	74.043278
399.797373	20.621681	74.048282
399.060940	25.174644	74.053287
398.765750	22.555195	74.058292
397.840433	25.110431	74.063297
396.794499	29.386302	74.068302
396.684062	27.647256	74.073306
395.869046	33.059509	74.078311
395.077562	20.066229	74.083316
394.206316	23.249895	74.088321
393.374934	30.082339	74.093326
393.538706	30.377886	74.098330
392.748416	26.681494	74.103335
391.850849	22.969083	74.108340
391.365188	31.870454	74.113345
390.615433	43.131873	74.118350
389.855228	25.898197	74.123354
388.594322	18.547556	74.128359
388.247870	36.984004	74.133364
388.022342	13.826092	74.138369
387.077726	35.883668	74.143374
386.982007	26.634917	74.148378
385.990251	36.386429	74.153383
385.467932	23.279306	74.158388
384.837012	31.869530	74.163393
383.645496	31.518486	74.168398
383.160957	26.450408	74.173402
382.229720	39.371200	74.178407
382.187587	30.213250	74.183412
381.704001	28.634579	74.188417
380.445768	39.516577	74.193422
379.993830	28.170612	74.198426
379.576714	30.562884	74.203431
378.593770	24.583964	74.208436
377.604543	29.366434	74.213441
377.201186	30.625917	74.218446
377.015093	29.020344	74.223450
376.119784	36.824856	74.228455
375.408627	32.832029	74.233460
374.873643	32.821049	74.238465
374.014823	34.616697	74.243470
373.142369	25.061234	74.248474
372.296489	35.588965	74.253479
371.924006	25.802460	74.258484
371.553361	35.398241	74.263489
370.966065	28.476401	74.268494
370.157141	31.052522	74.273498
369.257367	35.841243	74.278503
368.945216	43.013559	74.283508
368.053569	35.501588	74.288513
366.990411	40.369958	74.293518
366.611249	34.569202	74.298522
365.843659	18.885186	74.303527
365.737400	35.481026	74.308532
365.180370	35.686435	74.313537
363.704609	26.709621	74.318542
363.614701	34.540332	74.323546
362.729864	32.770152	74.328551
362.140408	30.412048	74.333556
361.382049	38.950052	74.338561
360.839450	28.399078	74.343566
360.369023	20.544053	74.348570
359.437123	29.784594	74.353575
358.884300	17.499152	74.358580
358.370124	31.616537	74.363585
357.777675	28.897814	74.368590
356.723393	20.440435	74.373594
355.975401	36.711208	74.378599
355.686096	38.863937	74.383604
355.111163	18.242084	74.388609
353.981519	13.194818	74.393614
353.192219	24.361613	74.398618
352.508935	31.263502	74.403623
352.293388	22.629900	74.408628
352.140276	21.585162	74.413633
350.995113	30.241565	74.418638
350.715590	22.513806	74.423642
349.765476	31.135976	74.428647
348.784166	32.864425	74.433652
347.946776	38.147803	74.438657
347.527736	27.602374	74.443662
347.139653	20.629878	74.448666
346.019702	30.546895	74.453671
344.809152	30.015989	74.458676
344.335404	22.355448	74.463681
344.328771	28.372129	74.468686
344.293177	27.792756	74.473690
343.549010	21.137182	74.478695
342.480427	30.828410	74.483700
341.977099	35.989174	74.488705
340.795632	29.613003	74.493710
340.096734	25.797995	74.498714
339.447563	35.282054	74.503719
338.855974	16.616577	74.508724
338.994408	31.809447	74.513729
337.551984	25.698775	74.518734
337.050130	13.883005	74.523738
336.221434	43.035266	74.528743
336.000836	24.860979	74.533748
334.883511	30.941122	74.538753
333.739357	39.523265	74.543758
334.000177	19.457320	74.548762
333.355169	17.754584	74.553767
332.545419	23.159704	74.558772
331.715155	28.878733	74.563777
331.004537	41.663463	74.568782
330.750513	11.368585	74.573786
329.710885	33.967972	74.578791
328.919629	38.466619	74.583796
328.468903	23.091642	74.588801
327.942307	20.504351	74.593806
327.003407	41.923989	74.598810
326.195756	26.973293	74.603815
325.696749	39.221287	74.608820
325.572352	19.334995	74.613825
324.188247	35.864824	74.618830
323.623638	33.047062	74.623834
322.630123	25.248596	74.628839
322.318464	35.531945	74.633844
322.215797	39.346890	74.638849
321.666468	34.315956	74.643854
320.720539	15.984480	74.648858
319.888430	23.379988	74.653863
319.227736	27.085174	74.658868
318.268792	21.115073	74.663873
317.274127	38.506877	74.668878
317.278941	18.563729	74.673882
316.701325	25.652196	74.678887
316.216725	39.509430	74.683892
315.864077	28.223351	74.688897
314.930346	33.321830	74.693902
314.268712	24.948544	74.698906
313.093275	34.426593	74.703911
312.666890	24.101529	74.708916
312.339322	32.676537	74.713921
310.834430	36.729136	74.718926
310.542087	22.710241	74.723930
309.717980	25.462252	74.728935
309.207369	25.846344	74.733940
308.720672	31.844918	74.738945
307.458315	32.787175	74.743950
307.177939	14.185651	74.748954
306.723393	26.866489	74.753959
306.381023	25.891337	74.758964
305.830448	29.001853	74.763969
304.368443	30.951994	74.768974
303.924072	30.693216	74.773978
303.730277	26.144911	74.778983
302.521666	31.875363	74.783988
301.770128	17.052932	74.788993
301.162845	32.271603	74.793998
300.959373	39.931191	74.799002
300.078568	24.069715	74.804007
299.185285	29.585922	74.809012
298.923698	30.540568	74.814017
298.155003	30.669346	74.819022
297.302691	25.814432	74.824026
296.398481	22.071582	74.829031
295.868173	22.840411	74.834036
295.636227	33.043250	74.839041
294.854242	37.338592	74.844046
294.149546	19.295089	74.849050
293.303410	29.734572	74.854055
292.633909	37.138869	74.859060
292.464725	18.708844	74.864065
291.117573	30.224740	74.869070
290.567792	27.303707	74.874074
289.910450	42.147195	74.879079
289.484302	30.347745	74.884084
289.119660	20.115346	74.889089
288.262229	42.794519	74.894094
287.575012	31.547574	74.899098
286.993603	21.195191	74.904103
286.077103	26.335082	74.909108
285.295072	39.399262	74.914113
284.411254	28.262497	74.919118
284.175170	20.154117	74.924122
283.489075	19.544387	74.929127
282.952616	32.173635	74.934132
282.249372	10.796470	74.939137
281.178047	48.764113	74.944142
281.339150	9.825062	74.949146
280.443342	42.736170	74.954151
279.453528	27.363552	74.959156
279.069666	21.684987	74.964161
278.167173	25.371953	74.969166
277.947637	24.200622	74.974170
277.092997	30.453370	74.979175
276.290652	31.309712	74.984180
275.886505	19.465771	74.989185
274.194735	39.053273	74.994190
273.948844	31.066292	74.999194
273.331538	18.594052	75.004199
272.710081	29.642659	75.009204
272.851273	22.089119	75.014209
271.939286	11.925043	75.019214
271.183685	40.438066	75.024218
270.769813	8.900913	75.029223
269.587432	49.167947	75.034228
268.632205	12.273800	75.039233
267.937354	20.131534	75.044238
267.780291	32.602551	75.049242
267.127536	3.754158	75.054247
266.185062	42.303601	75.059252
265.353111	10.604439	75.064257
264.854459	46.031968	75.069262
264.451807	11.060234	75.074266
263.883896	44.390561	75.079271
263.117051	11.265016	75.084276
262.780356	-7.980301	75.089281
261.948466	52.535849	75.094286
261.036358	13.141841	75.099290
260.052928	44.912672	75.104295
259.589923	14.056658	75.109300
259.329926	49.629070	75.114305
258.365274	35.742562	75.119310
257.691603	-1.942262	75.124314
256.789909	38.893397	75.129319
256.163068	40.991132	75.134324
256.213495	12.227757	75.139329
255.424022	18.377086	75.144334
254.353735	40.330147	75.149338
254.107336	9.794410	75.154343
253.255381	45.429624	75.159348
252.464544	9.382868	75.164353
251.680083	32.577062	75.169358
251.137851	14.777331	75.174362
250.808522	25.016184	75.179367
249.787714	26.186455	75.184372
249.412050	16.829396	75.189377
248.487716	25.620936	75.194382
248.003435	23.373824	75.199386
246.514372	20.541018	75.204391
245.827757	34.547135	75.209396
245.599709	25.439337	75.214401
245.005378	28.798096	75.219406
244.844702	28.330118	75.224410
244.452742	27.694016	75.229415
243.291491	23.992157	75.234420
242.829738	23.315144	75.239425
241.980246	33.181205	75.244430
241.189642	15.340647	75.249434
240.526772	25.394561	75.254439
239.446432	12.322832	75.259444
239.421141	13.399079	75.264449
239.040242	26.780913	75.269454
237.782800	18.821149	75.274458
237.340685	24.092007	75.279463
236.984911	30.165910	75.284468
236.358761	20.288998	75.289473
235.429308	22.211059	75.294478
234.411755	22.319603	75.299482
234.087374	33.735575	75.304487
232.829503	30.186305	75.309492
232.317369	18.566157	75.314497
232.118281	38.190122	75.319502
231.528633	13.633301	75.324506
230.884061	31.707273	75.329511
229.997020	26.009581	75.334516
229.297505	25.247475	75.339521
228.628557	24.920436	75.344526
228.520146	21.555355	75.349530
227.359308	40.809111	75.354535
226.675369	14.009282	75.359540
226.485509	31.963469	75.364545
225.066865	27.351810	75.369550
224.481459	25.936049	75.374554
223.893707	14.550296	75.379559
223.519246	48.993001	75.384564
223.361012	20.264458	75.389569
222.098887	25.777984	75.394574
221.441845	36.983651	75.399578
221.170601	24.513030	75.404583
220.255718	27.891353	75.409588
219.445392	21.681580	75.414593
218.306792	34.421009	75.419598
218.232134	21.745602	75.424602
217.598800	21.658877	75.429607
216.463855	32.573316	75.434612
216.030404	27.284264	75.439617
215.463188	29.115477	75.444622
214.959233	27.344560	75.449626
214.002557	27.695704	75.454631
212.955960	29.013593	75.459636
212.808008	11.786500	75.464641
212.259265	36.075299	75.469646
211.955875	31.754194	75.474650
211.094797	27.498336	75.479655
210.336745	27.030974	75.484660
209.861353	11.527529	75.489665
208.693790	28.920099	75.494670
207.862539	27.466266	75.499674
207.546486	17.751233	75.504679
206.834669	22.281396	75.509684
206.939687	22.699828	75.514689
205.723097	22.177838	75.519694
205.091701	14.324866	75.524698
204.438178	27.706008	75.529703
202.864726	34.190049	75.534708
202.471026	26.538861	75.539713
201.799808	33.546083	75.544718
201.783915	30.230905	75.549722
201.392460	29.022336	75.554727
200.500675	32.043771	75.559732
200.050119	24.466299	75.564737
199.086307	24.725551	75.569742
198.360084	25.326949	75.574746
197.302094	31.798204	75.579751
196.538695	17.417652	75.584756
196.385499	37.679223	75.589761
196.007588	22.122388	75.594766
195.414873	25.827803	75.599770
194.341551	19.902799	75.604775
193.675509	32.655206	75.609780
193.329667	12.790068	75.614785
191.753512	39.555879	75.619790
191.052804	33.532050	75.624794
190.936729	28.299635	75.629799
190.067160	22.361073	75.634804
190.079668	26.432024	75.639809
189.620509	25.795605	75.644814
188.658708	26.813002	75.649818
188.024501	31.952077	75.654823
187.150944	29.625117	75.659828
186.186001	19.444290	75.664833
185.163674	26.130619	75.669838
184.927384	23.527043	75.674842
184.772563	13.068852	75.679847
184.136945	21.604663	75.684852
183.508661	20.260399	75.689857
182.679880	20.223762	75.694862
182.039322	25.193549	75.699866
180.869658	20.315164	75.704871
180.047316	36.369168	75.709876
180.100571	26.655181	75.714881
179.320363	32.976511	75.719886
178.523918	23.331756	75.724890
177.864882	21.899363	75.729895
176.891160	30.042833	75.734900
176.644080	29.054085	75.739905
176.067148	34.797424	75.744910
175.241842	17.271491	75.749914
174.830653	35.016549	75.754919
173.690298	37.468960	75.759924
173.078299	9.068246	75.764929
172.084085	13.886268	75.769934
171.694772	28.007406	75.774938
171.595033	25.099807	75.779943
170.980777	18.576543	75.784948
170.102583	11.152409	75.789953
169.051845	21.730180	75.794958
168.547441	29.515002	75.799962
168.333701	7.542660	75.804967
167.230495	23.871647	75.809972
166.881907	35.324593	75.814977
165.782181	15.663219	75.819982
165.381068	39.086454	75.824986
164.857672	5.589464	75.829991
163.752577	8.842018	75.834996
163.429050	20.448641	75.840001
162.459739	20.839663	75.845006
161.539502	9.585784	75.850010
161.237583	30.260528	75.855015
160.706579	27.987770	75.860020
160.063588	19.591072	75.865025
159.566428	29.974950	75.870030
158.784754	30.094802	75.875034
158.038506	17.116500	75.880039
157.408300	22.562423	75.885044
156.555807	20.590062	75.890049
155.659991	28.948182	75.895054
154.979023	19.122616	75.900058
154.853774	18.005647	75.905063
154.459281	25.299893	75.910068
153.925651	24.587051	75.915073
152.836191	31.334555	75.920078
152.294741	16.666345	75.925082
151.288897	20.902801	75.930087
150.350719	20.970342	75.935092
150.056644	23.650513	75.940097
149.554025	25.151343	75.945102
149.338301	19.756639	75.950106
147.951605	25.774148	75.955111
147.109057	19.891217	75.960116
147.085279	21.158021	75.965121
146.502820	9.656347	75.970126
145.318845	26.941169	75.975130
144.518247	23.902478	75.980135
143.914214	9.457130	75.985140
143.618278	35.876928	75.990145
142.794598	18.656658	75.995150
141.801969	14.043363	76.000154
141.574913	18.463141	76.005159
141.052633	15.384810	76.010164
140.812580	18.601955	76.015169
139.556818	30.415558	76.020174
138.990104	34.443248	76.025178
138.461502	16.374903	76.030183
137.313479	8.795123	76.035188
137.072542	24.425288	76.040193
136.399459	10.175442	76.045198
135.596962	37.136440	76.050202
134.757855	15.098235	76.055207
133.752420	45.958016	76.060212
133.884409	10.339760	76.065217
133.077654	20.422936	76.070222
132.438181	30.257113	76.075226
131.663329	16.597458	76.080231
130.931247	25.408837	76.085236
130.334626	29.329340	76.090241
129.016504	27.617293	76.095246
128.407403	8.669305	76.100250
128.005258	21.531012	76.105255
127.602429	30.513811	76.110260
127.696135	27.081821	76.115265
126.205532	18.807663	76.120270
125.389259	39.695302	76.125274
125.043174	20.479876	76.130279
124.706174	21.913306	76.135284
124.166207	17.467526	76.140289
123.157957	25.673281	76.145294
122.566952	24.822948	76.150298
121.791913	10.307109	76.155303
120.331434	37.607967	76.160308
120.066965	28.715718	76.165313
119.237119	30.897887	76.170318
119.023475	26.114668	76.175322
119.058091	20.028818	76.180327
117.654948	21.950759	76.185332
116.847080	16.664665	76.190337
116.374615	29.201724	76.195342
115.791484	17.697008	76.200346
115.669766	17.430972	76.205351
114.776815	28.011989	76.210356
113.897684	15.203119	76.215361
112.716847	26.944863	76.220366
111.786122	24.739004	76.225370
111.407922	18.599138	76.230375
110.548338	32.740073	76.235380
110.679983	23.421998	76.240385
110.208860	24.126239	76.245390
109.897708	13.491153	76.250394
108.883607	18.438517	76.255399
107.948723	20.118656	76.260404
107.125970	15.353720	76.265409
106.401695	23.602503	76.270414
105.691161	25.784574	76.275418
105.316205	17.214282	76.280423
104.476700	16.966508	76.285428
103.605319	37.989081	76.290433
103.082825	23.175945	76.295438
102.915749	21.606788	76.300442
102.041730	17.149627	76.305447
101.032471	24.683817	76.310452
100.445903	29.550403	76.315457
99.887032	15.802713	76.320462
99.539121	15.433982	76.325466
98.621354	31.829614	76.330471
97.948112	24.267178	76.335476
97.448115	19.636848	76.340481
96.622396	31.755608	76.345486
95.661843	24.537007	76.350490
95.390810	6.005030	76.355495
94.139869	35.743386	76.360500
94.159211	24.528933	76.365505
93.655865	22.538766	76.370510
92.254271	21.295757	76.375514
92.137547	12.268010	76.380519
91.490731	24.924325	76.385524
90.748931	18.077673	76.390529
89.892530	23.911312	76.395534
89.260927	20.907192	76.400538
88.996143	26.105641	76.405543
87.783580	26.045082	76.410548
87.003655	20.475443	76.415553
86.640019	25.554046	76.420558
85.963024	27.456404	76.425562
85.594700	19.984115	76.430567
84.443062	25.956291	76.435572
83.924303	26.486797	76.440577
83.694989	27.105180	76.445582
82.880779	24.373012	76.450586
82.383843	13.964661	76.455591
81.003629	25.970003	76.460596
80.687738	22.622250	76.465601
80.557824	36.052375	76.470606
79.346465	28.143695	76.475610
78.742594	17.599442	76.480615
77.955878	23.630116	76.485620
77.700529	28.081217	76.490625
76.638564	26.065021	76.495630
75.616972	35.378289	76.500634
75.390658	21.643801	76.505639
74.935322	28.107302	76.510644
74.586549	11.945096	76.515649
73.403617	27.391181	76.520654
72.909141	28.055002	76.525658
72.682102	19.111072	76.530663
71.438781	21.655633	76.535668
70.846906	29.848624	76.540673
69.976660	28.598163	76.545678
69.320399	36.071349	76.550682
69.305559	20.131833	76.555687
67.910134	27.134722	76.560692
67.580138	20.635542	76.565697
66.825206	33.892538	76.570702
66.285722	22.932770	76.575706
65.162733	20.150507	76.580711
64.590014	28.845032	76.585716
64.296084	25.452781	76.590721
63.921064	24.531754	76.595726
63.056026	31.431148	76.600730
62.197331	27.499798	76.605735
61.237129	28.731438	76.610740
61.089526	28.450610	76.615745
60.831073	22.912932	76.620750
59.519033	31.469908	76.625754
58.751541	28.202057	76.630759
58.312433	24.905492	76.635764
58.116722	20.128885	76.640769
56.857448	17.570194	76.645774
55.878442	35.068353	76.650778
55.889973	24.626225	76.655783
55.184105	18.923372	76.660788
54.131431	26.445579	76.665793
53.243818	27.109023	76.670798
52.946395	24.133616	76.675802
52.954723	18.545514	76.680807
51.748568	31.393531	76.685812
51.104075	28.542852	76.690817
50.575054	26.397528	76.695822
49.745693	27.278749	76.700826
49.110549	23.791114	76.705831
48.329208	30.543133	76.710836
47.918978	14.253549	76.715841
46.969383	17.996982	76.720846
46.011085	34.936794	76.725850
45.544806	21.283155	76.730855
44.893875	29.463493	76.735860
44.719311	27.070847	76.740865
44.157340	28.212181	76.745870
42.980020	30.654776	76.750874
42.636095	24.474765	76.755879
41.884938	38.368210	76.760884
40.644440	23.565529	76.765889
40.169823	26.260311	76.770894
39.392489	29.476421	76.775898
39.501185	29.033304	76.780903
38.562998	25.409510	76.785908
37.844154	22.312091	76.790913
37.292178	24.322248	76.795918
36.584626	26.234222	76.800922
36.094951	22.289762	76.805927
35.080889	24.353111	76.810932
34.354581	20.312359	76.815937
33.856269	20.867997	76.820942
33.235474	27.690602	76.825946
32.406864	25.143662	76.830951
31.537981	27.127094	76.835956
31.287141	28.567294	76.840961
30.835815	29.183244	76.845966
30.168979	22.269469	76.850970
29.654075	23.426953	76.855975
28.689089	23.669114	76.860980
27.725458	24.327345	76.865985
26.888168	16.562459	76.870990
26.476392	27.282787	76.875994
26.378305	22.041215	76.880999
25.393403	29.161569	76.886004
24.401179	16.684570	76.891009
23.931194	21.046909	76.896014
22.963146	17.396349	76.901018
22.880985	12.592179	76.906023
22.048659	29.283257	76.911028
21.164419	27.621914	76.916033
20.623618	17.718858	76.921038
20.196393	16.260578	76.926042
19.270391	22.630424	76.931047
17.960062	34.134258	76.936052
17.817820	19.665762	76.941057
17.412894	18.820470	76.946062
16.835106	24.456743	76.951066
16.517917	14.713556	76.956071
15.259373	22.708545	76.961076
14.613493	18.547747	76.966081
14.126280	18.365236	76.971086
13.346000	23.824085	76.976090
12.693979	22.843172	76.981095
11.813355	24.394853	76.986100
11.476778	18.259408	76.991105
11.187735	23.608376	76.996110
9.740846	28.473426	77.001114
9.259243	21.046027	77.006119
8.744853	35.056242	77.011124
8.430458	28.478895	77.016129
7.978634	26.285003	77.021134
7.301456	31.535038	77.026139
6.290547	20.563753	77.031143
4.888221	26.755702	77.036148
4.220762	20.986820	77.041153
3.804119	19.541047	77.046158