Mon Mar 08 20:16:12 2021

Number of Points = 14582

Depth (nm)	Load (N)	Time (s)
-0.750697	103.107555	0.000000
-0.941205	88.274600	0.005005
-1.334468	46.737130	0.010010
-4.445875	28.360224	0.015014
-8.843773	25.945842	0.020019
-13.686554	38.658047	0.025024
-18.212130	21.500143	0.030029
-22.367117	17.508052	0.035034
-26.724273	29.147831	0.040038
-30.475278	32.048305	0.045043
-34.131931	24.703234	0.050048
-37.568127	22.212767	0.055053
-40.888934	27.884511	0.060058
-44.684280	27.408194	0.065062
-48.619614	15.856461	0.070067
-52.729398	29.516167	0.075072
-56.573451	21.144549	0.080077
-60.028630	24.997589	0.085082
-64.022330	32.643678	0.090086
-67.498434	25.556841	0.095091
-71.318936	33.694090	0.100096
-75.496675	28.706005	0.105101
-78.941473	26.177548	0.110106
-82.778063	34.662708	0.115110
-86.217704	27.067072	0.120115
-90.003626	25.351508	0.125120
-93.953243	19.117636	0.130125
-97.564454	9.411214	0.135130
-101.441834	30.235307	0.140134
-105.140255	21.730158	0.145139
-109.138383	27.139496	0.150144
-112.793117	32.500364	0.155149
-116.342803	18.676499	0.160154
-120.533371	20.598646	0.165158
-124.225206	26.241392	0.170163
-128.017244	15.846407	0.175168
-132.035947	27.741419	0.180173
-134.996091	24.060316	0.185178
-138.777181	17.175207	0.190182
-142.439485	19.325316	0.195187
-146.251344	31.185772	0.200192
-150.204295	6.844200	0.205197
-154.224714	3.985113	0.210202
-158.917382	41.423572	0.215206
-162.402082	23.007132	0.220211
-165.750993	14.777451	0.225216
-169.512168	26.891604	0.230221
-172.939957	29.340203	0.235226
-176.686378	16.962250	0.240230
-180.627519	34.981990	0.245235
-184.084232	31.438529	0.250240
-187.875917	8.451021	0.255245
-191.647898	41.586090	0.260250
-196.168803	27.972520	0.265254
-199.421071	5.791444	0.270259
-203.132135	46.416217	0.275264
-206.946213	11.629720	0.280269
-209.956446	21.474870	0.285274
-214.612387	29.592701	0.290278
-218.209209	28.911524	0.295283
-222.073116	20.054536	0.300288
-225.686452	28.778645	0.305293
-229.493875	0.853526	0.310298
-233.363531	22.051841	0.315302
-237.108824	31.449835	0.320307
-240.914432	22.116831	0.325312
-244.616869	42.881681	0.330317
-247.925025	22.686923	0.335322
-252.005539	26.031376	0.340326
-255.654791	31.628100	0.345331
-259.462627	15.472544	0.350336
-263.213279	43.935311	0.355341
-266.658740	20.559955	0.360346
-271.040739	25.871561	0.365350
-274.886358	30.902036	0.370355
-278.495545	20.870746	0.375360
-282.462781	34.112275	0.380365
-285.635537	14.802655	0.385370
-289.288288	30.813363	0.390374
-293.090928	21.765380	0.395379
-296.964166	23.093172	0.400384
-300.820384	26.979023	0.405389
-304.974461	12.040942	0.410394
-308.722643	25.282226	0.415398
-312.436376	35.479477	0.420403
-315.779525	19.511592	0.425408
-319.796546	19.298158	0.430413
-323.472887	34.551074	0.435418
-327.677949	24.499874	0.440422
-331.148451	17.194945	0.445427
-334.963763	24.321008	0.450432
-338.270631	24.063619	0.455437
-341.784145	28.487714	0.460442
-346.094388	30.563383	0.465446
-349.769020	21.097700	0.470451
-353.582501	20.164332	0.475456
-357.460202	23.662648	0.480461
-361.095730	22.773416	0.485466
-365.186117	31.807254	0.490470
-368.766194	23.127534	0.495475
-372.334150	26.836599	0.500480
-376.160279	35.063505	0.505485
-379.714705	19.807488	0.510490
-383.820035	25.450406	0.515494
-387.250619	23.606049	0.520499
-391.169794	37.626908	0.525504
-395.336898	26.046555	0.530509
-398.733979	19.188864	0.535514
-402.709361	33.234478	0.540518
-406.260212	23.468447	0.545523
-410.139581	34.346667	0.550528
-413.923619	38.016185	0.555533
-417.131434	21.686254	0.560538
-421.498186	29.999547	0.565542
-425.357369	28.119610	0.570547
-428.649789	35.187556	0.575552
-432.851504	38.740884	0.580557
-436.095802	27.021141	0.585562
-440.024180	41.335258	0.590566
-443.376805	28.860175	0.595571
-447.665735	25.823703	0.600576
-451.706756	36.406127	0.605581
-455.108321	21.479033	0.610586
-459.125774	34.629507	0.615590
-462.703023	31.756936	0.620595
-466.342894	24.835620	0.625600
-470.321245	36.762559	0.630605
-473.634693	28.513473	0.635610
-478.011112	15.244816	0.640614
-481.806996	25.218898	0.645619
-485.529192	26.448760	0.650624
-489.300439	27.558738	0.655629
-492.643732	24.916912	0.660634
-496.323246	35.328140	0.665638
-499.753642	14.524167	0.670643
-503.817601	18.326827	0.675648
-508.193934	26.059950	0.680653
-511.717081	28.886923	0.685658
-515.817330	30.781135	0.690662
-519.299378	25.452521	0.695667
-522.704139	33.990788	0.700672
-526.418757	41.435353	0.705677
-530.431471	19.002535	0.710682
-534.279436	38.108530	0.715686
-537.945629	32.594905	0.720691
-541.874898	37.090421	0.725696
-545.684280	31.263815	0.730701
-549.134645	24.395936	0.735706
-552.753035	42.445087	0.740710
-556.548533	27.074910	0.745715
-560.272094	17.779804	0.750720
-564.169174	17.325291	0.755725
-567.917583	21.571200	0.760730
-572.000391	40.104532	0.765734
-575.365586	32.373174	0.770739
-579.473302	16.901546	0.775744
-583.640370	43.896981	0.780749
-586.893921	30.007649	0.785754
-590.853396	39.782548	0.790758
-594.186934	42.275027	0.795763
-598.102115	19.495626	0.800768
-601.552358	41.475807	0.805773
-605.446973	31.865921	0.810778
-609.519641	27.078036	0.815782
-613.320798	41.178138	0.820787
-617.177817	35.017088	0.825792
-621.180984	28.117791	0.830797
-624.142343	29.882278	0.835802
-627.913205	28.061098	0.840806
-632.037785	26.055179	0.845811
-635.606915	32.880619	0.850816
-639.796935	36.345710	0.855821
-643.073271	20.072802	0.860826
-647.197912	29.897823	0.865830
-650.798498	25.176503	0.870835
-654.223277	24.167325	0.875840
-658.669431	20.922992	0.880845
-661.926088	21.982561	0.885850
-665.731864	24.686194	0.890854
-669.586312	19.485115	0.895859
-673.065077	20.438273	0.900864
-677.200856	30.295082	0.905869
-680.799026	28.088455	0.910874
-684.955629	16.149039	0.915878
-688.458709	19.170164	0.920883
-691.967690	9.301724	0.925888
-695.870523	23.673620	0.930893
-699.515453	22.302326	0.935898
-703.501901	30.634183	0.940902
-707.133518	21.632109	0.945907
-711.196986	38.366559	0.950912
-714.632481	30.424314	0.955917
-718.282194	13.922636	0.960922
-722.750485	30.530989	0.965926
-726.225002	26.035626	0.970931
-729.685872	16.877007	0.975936
-733.579483	27.576651	0.980941
-737.219700	25.589702	0.985946
-741.477385	28.028232	0.990950
-744.948803	24.498995	0.995955
-748.397807	26.210688	1.000960
-752.383000	27.645407	1.005965
-755.922268	17.534343	1.010970
-759.483763	11.961776	1.015974
-763.663151	18.938533	1.020979
-766.999821	28.164773	1.025984
-771.172541	32.735831	1.030989
-774.741508	13.510790	1.035994
-779.020869	33.621124	1.040998
-782.727024	32.248706	1.046003
-786.015166	16.293277	1.051008
-790.238421	16.637104	1.056013
-793.520865	24.068173	1.061018
-797.539360	29.313157	1.066022
-801.342152	21.466023	1.071027
-805.034755	24.951234	1.076032
-809.070391	42.085056	1.081037
-812.251728	30.029408	1.086042
-816.252905	28.235883	1.091046
-820.033752	23.368617	1.096051
-823.815750	38.713223	1.101056
-827.732057	34.515690	1.106061
-831.401182	15.795569	1.111066
-835.264187	40.964110	1.116070
-838.638164	27.862328	1.121075
-842.497766	31.136192	1.126080
-846.495694	33.191218	1.131085
-850.031063	28.494476	1.136090
-854.280326	22.710324	1.141094
-857.912469	29.613958	1.146099
-861.600318	29.623187	1.151104
-865.346240	39.747545	1.156109
-868.512629	24.271049	1.161114
-872.136291	33.577998	1.166118
-876.112826	27.810206	1.171123
-880.141118	21.404201	1.176128
-884.355602	32.740375	1.181133
-888.182485	31.231320	1.186138
-891.734312	22.767102	1.191142
-894.923468	20.853358	1.196147
-898.535302	17.047208	1.201152
-902.651736	19.722040	1.206157
-906.512303	21.334194	1.211162
-910.702582	30.244548	1.216166
-914.336308	21.288879	1.221171
-917.842159	23.512911	1.226176
-921.868222	26.725214	1.231181
-925.376747	23.568005	1.236186
-929.052917	24.723396	1.241190
-933.177457	26.568594	1.246195
-936.741609	17.992892	1.251200
-940.366580	20.070436	1.256205
-944.014845	21.043208	1.261210
-947.992419	25.173394	1.266214
-951.701835	24.088748	1.271219
-955.015267	17.820867	1.276224
-958.973060	30.279811	1.281229
-963.063165	21.649488	1.286234
-967.195575	29.801696	1.291238
-970.488796	23.991034	1.296243
-973.889690	19.414899	1.301248
-977.942603	27.049831	1.306253
-981.856832	19.671795	1.311258
-985.638875	19.291040	1.316262
-989.436306	27.780769	1.321267
-992.991427	12.820762	1.326272
-997.089202	18.714207	1.331277
-1000.689971	25.742330	1.336282
-1004.427369	29.223974	1.341286
-1008.087907	27.258045	1.346291
-1011.814284	22.901160	1.351296
-1015.702340	34.715162	1.356301
-1019.450389	34.311680	1.361306
-1023.259668	30.639793	1.366310
-1027.024351	15.595093	1.371315
-1030.261876	28.856662	1.376320
-1034.627508	38.157942	1.381325
-1038.175675	34.094266	1.386330
-1042.180246	26.426456	1.391334
-1046.033970	25.396577	1.396339
-1049.547998	16.365225	1.401344
-1053.144084	31.976861	1.406349
-1057.035024	13.579601	1.411354
-1060.921169	31.930839	1.416358
-1064.548060	35.057464	1.421363
-1067.916968	24.851850	1.426368
-1071.756130	24.874574	1.431373
-1075.875970	20.631186	1.436378
-1079.689194	29.199266	1.441382
-1083.458611	28.778806	1.446387
-1087.183651	16.067867	1.451392
-1091.085005	23.582555	1.456397
-1094.424872	21.584393	1.461402
-1098.555357	35.823022	1.466406
-1102.286056	17.766031	1.471411
-1105.987074	41.316449	1.476416
-1110.025007	7.177808	1.481421
-1113.232575	30.631940	1.486426
-1117.034876	14.642600	1.491430
-1121.351463	36.973286	1.496435
-1124.325823	21.466466	1.501440
-1128.652105	4.111889	1.506445
-1132.049908	20.850858	1.511450
-1135.980772	2.198397	1.516454
-1139.709834	40.551730	1.521459
-1143.447928	3.940058	1.526464
-1147.365045	48.954001	1.531469
-1150.847142	18.993362	1.536474
-1155.011650	8.535164	1.541478
-1158.960145	21.350860	1.546483
-1162.567393	23.365991	1.551488
-1166.422372	35.958610	1.556493
-1169.492515	20.031980	1.561498
-1173.401580	29.752421	1.566502
-1177.387953	35.160040	1.571507
-1180.905653	14.204045	1.576512
-1184.917357	36.465555	1.581517
-1189.110986	31.726440	1.586522
-1192.881117	24.030855	1.591526
-1196.234609	33.440112	1.596531
-1199.435829	21.441844	1.601536
-1203.454245	18.292537	1.606541
-1206.860300	19.004633	1.611546
-1211.430428	14.327385	1.616550
-1215.345730	47.655367	1.621555
-1218.762497	15.237191	1.626560
-1222.686831	16.396482	1.631565
-1226.424535	40.146876	1.636570
-1230.075639	36.197734	1.641574
-1233.840694	23.916033	1.646579
-1237.424306	37.179634	1.651584
-1241.501904	22.232687	1.656589
-1244.980701	37.489962	1.661594
-1248.626416	12.833294	1.666598
-1252.334184	39.814548	1.671603
-1256.109213	25.438896	1.676608
-1260.481803	23.229380	1.681613
-1264.117138	22.436128	1.686618
-1267.792818	30.670280	1.691622
-1271.427681	23.410458	1.696627
-1275.022167	7.396041	1.701632
-1278.939293	38.007534	1.706637
-1282.555630	42.064701	1.711642
-1286.667034	28.340545	1.716646
-1290.322879	13.610031	1.721651
-1293.571758	19.186788	1.726656
-1297.965499	14.577671	1.731661
-1301.791552	21.301699	1.736666
-1305.348961	23.354799	1.741670
-1308.966324	28.921175	1.746675
-1312.497950	32.318334	1.751680
-1316.559649	22.553546	1.756685
-1320.049581	12.918012	1.761690
-1324.163811	21.165669	1.766694
-1328.135682	27.736477	1.771699
-1331.955099	24.604426	1.776704
-1335.475871	31.987637	1.781709
-1339.087563	40.016134	1.786714
-1342.871416	12.664904	1.791718
-1347.032858	38.936798	1.796723
-1350.067511	23.413151	1.801728
-1354.188293	30.955501	1.806733
-1357.822035	17.352137	1.811738
-1361.616730	35.239791	1.816742
-1365.067534	25.334731	1.821747
-1368.980454	17.446285	1.826752
-1372.981539	4.888844	1.831757
-1376.704124	24.731243	1.836762
-1380.396432	25.584024	1.841766
-1384.198449	17.971138	1.846771
-1388.026769	13.963904	1.851776
-1391.953326	16.916668	1.856781
-1395.629077	24.944457	1.861786
-1399.054052	16.205316	1.866790
-1403.170371	14.609426	1.871795
-1406.956793	11.145823	1.876800
-1410.502193	11.740189	1.881805
-1414.815987	28.284004	1.886810
-1417.762647	25.225244	1.891814
-1421.791366	26.595531	1.896819
-1425.224826	23.319853	1.901824
-1429.290238	17.537316	1.906829
-1433.009467	13.019153	1.911834
-1437.043012	33.382898	1.916838
-1441.066457	10.728120	1.921843
-1444.330895	28.899962	1.926848
-1448.365989	26.685652	1.931853
-1452.131328	34.652188	1.936858
-1455.391468	4.279747	1.941862
-1459.588778	48.162622	1.946867
-1463.262109	19.179265	1.951872
-1467.450790	35.830866	1.956877
-1470.616365	30.252795	1.961882
-1474.631302	13.369416	1.966886
-1478.204945	34.233544	1.971891
-1481.862499	23.448806	1.976896
-1485.837764	39.224252	1.981901
-1489.287909	17.841700	1.986906
-1493.072260	29.824317	1.991910
-1497.197016	33.655743	1.996915
-1500.943796	22.294068	2.006912
-1502.370068	30.369173	2.016909
-1499.563872	16.098712	2.026906
-1496.335040	26.027139	2.036902
-1494.407437	34.867723	2.046899
-1492.875264	27.001325	2.056896
-1490.745134	19.400733	2.066893
-1488.817471	22.210191	2.076890
-1487.273693	21.160893	2.086886
-1485.025494	15.829123	2.096883
-1483.166619	30.669208	2.106880
-1480.961318	21.198307	2.116877
-1479.211703	17.012084	2.126874
-1477.701700	27.228393	2.136870
-1475.645530	19.098119	2.146867
-1473.412697	16.716488	2.156864
-1471.684517	19.654210	2.166861
-1469.709290	29.827613	2.176858
-1468.286628	14.605646	2.186854
-1465.970475	18.622295	2.196851
-1464.337480	18.918097	2.206848
-1462.205822	23.119017	2.216845
-1460.354365	19.347520	2.226842
-1458.288425	23.587385	2.236838
-1456.735119	22.050304	2.246835
-1454.822508	22.959714	2.256832
-1452.883092	17.323755	2.266829
-1451.064946	19.276109	2.276826
-1449.139550	19.176186	2.286822
-1447.408738	25.937426	2.296819
-1445.293981	28.240161	2.306816
-1443.362263	12.622517	2.316813
-1441.625280	27.171126	2.326810
-1439.883752	21.503705	2.336806
-1437.742541	20.382472	2.346803
-1436.123726	18.426000	2.356800
-1433.997905	17.629314	2.366797
-1432.090145	15.486069	2.376794
-1430.456939	14.930874	2.386790
-1428.278454	23.215071	2.396787
-1426.527187	15.231541	2.406784
-1424.697178	20.462820	2.416781
-1422.526388	15.036140	2.426778
-1420.830944	22.474063	2.436774
-1418.948971	23.246315	2.446771
-1417.355905	26.644625	2.456768
-1415.146331	20.997020	2.466765
-1413.427653	15.265388	2.476762
-1411.677579	23.997106	2.486758
-1409.732890	25.990811	2.496755
-1407.283333	8.252027	2.506752
-1405.890743	25.094577	2.516749
-1403.863623	11.739937	2.526746
-1402.341050	17.694611	2.536742
-1400.459815	10.288670	2.546739
-1398.306358	14.751403	2.556736
-1396.130412	24.101748	2.566733
-1394.451521	17.053440	2.576730
-1392.815812	15.894759	2.586726
-1390.739182	27.543996	2.596723
-1389.178892	15.503476	2.606720
-1387.019051	15.457646	2.616717
-1384.975815	23.139901	2.626714
-1383.281908	14.240390	2.636710
-1381.464220	23.310231	2.646707
-1379.611597	23.263065	2.656704
-1377.564298	29.841080	2.666701
-1375.775300	21.712603	2.676698
-1373.799547	23.706103	2.686694
-1372.207883	16.741240	2.696691
-1370.447967	21.178584	2.706688
-1367.974992	21.426832	2.716685
-1366.383441	19.610551	2.726682
-1364.603615	26.840820	2.736678
-1362.578850	14.433882	2.746675
-1360.730433	28.484766	2.756672
-1358.560067	19.329013	2.766669
-1356.991172	17.971067	2.776666
-1355.400039	20.651365	2.786662
-1353.440523	19.770855	2.796659
-1351.247706	19.356649	2.806656
-1349.381935	31.698056	2.816653
-1347.624442	28.140615	2.826650
-1345.796423	15.061023	2.836646
-1343.858632	35.165063	2.846643
-1342.220662	20.653891	2.856640
-1339.919711	18.468309	2.866637
-1338.074050	18.968565	2.876634
-1336.497139	15.593186	2.886630
-1334.445883	30.642606	2.896627
-1332.536427	24.618404	2.906624
-1330.765360	13.020987	2.916621
-1328.933737	24.052708	2.926618
-1326.895712	36.227632	2.936614
-1325.144505	29.298831	2.946611
-1323.301876	24.998363	2.956608
-1321.303504	18.325251	2.966605
-1319.417266	24.674906	2.976602
-1317.503725	18.896362	2.986598
-1315.871590	21.050690	2.996595
-1313.622289	24.876111	3.006592
-1311.911591	10.264911	3.016589
-1309.834618	22.252042	3.026586
-1308.184231	15.154672	3.036582
-1306.588053	24.528434	3.046579
-1304.565976	10.331579	3.056576
-1302.448759	22.364378	3.066573
-1300.710774	22.608760	3.076570
-1298.852860	23.683360	3.086566
-1296.827346	12.986225	3.096563
-1295.093887	22.642738	3.106560
-1293.224957	13.238466	3.116557
-1291.268281	14.507249	3.126554
-1289.215478	19.838767	3.136550
-1287.589987	5.858545	3.146547
-1285.945782	15.876687	3.156544
-1283.666851	9.706563	3.166541
-1281.952442	5.916087	3.176538
-1280.165657	17.839168	3.186534
-1278.119687	22.852867	3.196531
-1276.433490	10.815945	3.206528
-1274.281710	15.023298	3.216525
-1272.411813	16.798580	3.226522
-1270.562214	17.729280	3.236518
-1268.775355	15.188703	3.246515
-1267.089522	19.715349	3.256512
-1264.894408	12.060344	3.266509
-1262.980129	18.610807	3.276506
-1261.213329	17.418608	3.286502
-1259.334713	11.149947	3.296499
-1257.698690	25.618571	3.306496
-1256.026421	11.978217	3.316493
-1253.707598	20.443805	3.326490
-1251.790664	15.932569	3.336486
-1250.213270	23.228483	3.346483
-1247.854239	14.757846	3.356480
-1246.344368	19.757895	3.366477
-1244.396343	19.433485	3.376474
-1242.606557	33.722800	3.386470
-1240.110878	19.278104	3.396467
-1238.985593	22.831918	3.406464
-1237.001015	13.557590	3.416461
-1234.719355	10.702616	3.426458
-1233.076966	3.848140	3.436454
-1231.713067	33.079769	3.446451
-1229.571993	15.733098	3.456448
-1227.365178	9.615613	3.466445
-1225.370415	20.496594	3.476442
-1223.770110	19.155815	3.486438
-1221.965002	9.466566	3.496435
-1220.166466	25.600146	3.506432
-1217.967784	12.579741	3.516429
-1216.159212	24.554658	3.526426
-1214.313024	18.535934	3.536422
-1212.490037	18.490486	3.546419
-1210.535908	27.988618	3.556416
-1208.629872	25.171665	3.566413
-1206.951263	13.882783	3.576410
-1205.325890	23.624557	3.586406
-1203.003621	21.004676	3.596403
-1201.084631	18.218813	3.606400
-1199.130824	21.171169	3.616397
-1197.607602	21.456307	3.626394
-1195.559160	12.618601	3.636390
-1193.769235	21.681998	3.646387
-1191.732920	16.701741	3.656384
-1190.023633	16.510304	3.666381
-1187.975463	20.450130	3.676378
-1185.941762	14.702985	3.686374
-1184.192735	17.746534	3.696371
-1182.338365	17.099290	3.706368
-1180.924122	22.061007	3.716365
-1178.756129	15.180883	3.726362
-1176.737314	16.384564	3.736358
-1174.913374	19.386138	3.746355
-1173.113751	19.079215	3.756352
-1171.305373	16.510006	3.766349
-1169.145380	18.352638	3.776346
-1167.651359	18.374065	3.786342
-1165.464699	15.229641	3.796339
-1163.653358	11.992118	3.806336
-1161.561299	9.778555	3.816333
-1159.844837	18.834787	3.826330
-1158.212386	20.008725	3.836326
-1156.325447	25.417429	3.846323
-1154.421168	16.778067	3.856320
-1152.577124	21.486319	3.866317
-1150.477881	22.070885	3.876314
-1148.606727	10.156017	3.886310
-1146.773994	10.206949	3.896307
-1144.951777	18.922614	3.906304
-1143.261812	25.835892	3.916301
-1141.030462	25.068377	3.926298
-1139.158681	7.545403	3.936294
-1137.350509	30.401769	3.946291
-1135.661208	26.294904	3.956288
-1133.583056	14.190624	3.966285
-1131.786490	25.515482	3.976282
-1129.826642	27.060194	3.986278
-1128.028194	24.650488	3.996275
-1126.281150	20.970151	4.006272
-1124.330669	17.345688	4.016269
-1122.236493	19.018906	4.026266
-1120.384283	14.516548	4.036262
-1119.036156	20.810364	4.046259
-1116.703986	28.782955	4.056256
-1114.803717	29.571476	4.066253
-1113.055231	19.114565	4.076250
-1111.243156	17.138450	4.086246
-1108.890849	17.976236	4.096243
-1107.541473	17.692442	4.106240
-1105.528079	21.549493	4.116237
-1103.755907	26.581893	4.126234
-1101.916054	25.376549	4.136230
-1099.822993	24.435418	4.146227
-1097.981827	20.110092	4.156224
-1095.795032	19.832870	4.166221
-1094.444659	21.910859	4.176218
-1092.474393	20.749394	4.186214
-1090.468882	27.170168	4.196211
-1088.449782	14.270162	4.206208
-1086.892631	21.267880	4.216205
-1084.913557	17.910434	4.226202
-1082.868497	12.126822	4.236198
-1081.311728	18.589380	4.246195
-1079.324154	21.989565	4.256192
-1077.090661	22.150122	4.266189
-1075.591945	17.952214	4.276186
-1073.596862	16.207364	4.286182
-1071.644430	23.062928	4.296179
-1069.952675	16.587467	4.306176
-1067.966770	20.352640	4.316173
-1065.756548	17.073494	4.326170
-1064.320927	25.787915	4.336166
-1062.646728	26.557378	4.346163
-1060.535932	25.345044	4.356160
-1058.494871	20.130468	4.366157
-1056.590848	16.576643	4.376154
-1055.082919	20.735620	4.386150
-1053.024747	12.892714	4.396147
-1050.911046	16.058029	4.406144
-1049.005055	19.450765	4.416141
-1047.296139	17.915903	4.426138
-1045.423984	28.769311	4.436134
-1043.591348	23.952792	4.446131
-1041.634259	17.150723	4.456128
-1040.050390	17.473629	4.466125
-1038.065959	18.097184	4.476122
-1036.143405	13.762047	4.486118
-1033.933901	14.861151	4.496115
-1032.249465	26.342969	4.506112
-1030.502015	21.641130	4.516109
-1028.737182	21.120424	4.526106
-1026.658813	26.010766	4.536102
-1024.717936	23.444157	4.546099
-1022.976445	18.173317	4.556096
-1021.252674	16.620311	4.566093
-1019.092386	26.838757	4.576090
-1017.287445	20.667310	4.586086
-1015.588123	22.132213	4.596083
-1013.464436	25.761725	4.606080
-1011.503148	21.848274	4.616077
-1009.733650	26.860654	4.626074
-1008.076773	24.497360	4.636070
-1006.033842	15.307023	4.646067
-1004.456416	24.854537	4.656064
-1002.416674	25.464542	4.666061
-1000.437147	16.129622	4.676058
-998.429168	19.837646	4.686054
-996.599684	28.155998	4.696051
-994.778208	29.135627	4.706048
-992.904490	29.060134	4.716045
-991.038472	24.836694	4.726042
-989.070617	18.822360	4.736038
-987.276152	23.080818	4.746035
-985.425275	23.629466	4.756032
-983.537244	19.156214	4.766029
-981.602267	16.783202	4.776026
-979.616756	24.497185	4.786022
-978.154222	21.996053	4.796019
-975.996996	20.907413	4.806016
-974.149835	22.459225	4.816013
-972.560856	19.994715	4.826010
-970.424109	20.802378	4.836006
-968.410204	27.240870	4.846003
-966.562507	24.490274	4.856000
-964.732694	25.699103	4.865997
-962.849899	19.872063	4.875994
-961.008009	34.584331	4.885990
-959.269485	26.609458	4.895987
-957.351214	23.276046	4.905984
-955.059804	25.610990	4.915981
-953.636451	32.885978	4.925978
-952.035851	26.628835	4.935974
-950.036065	19.524765	4.945971
-947.961990	31.683253	4.955968
-945.878575	28.523956	4.965965
-943.683127	26.491404	4.975962
-942.268786	24.435337	4.985958
-940.261731	26.076866	4.995955
-938.423148	17.020298	5.005952
-936.594202	17.724060	5.015949
-934.730387	29.090447	5.025946
-933.001429	20.297707	5.035942
-931.060372	25.757950	5.045939
-928.958726	29.567898	5.055936
-927.499904	17.722254	5.065933
-925.528790	21.703062	5.075930
-923.456203	26.970190	5.085926
-921.448124	22.635674	5.095923
-919.648970	24.919892	5.105920
-917.968727	19.466297	5.115917
-916.150898	21.600700	5.125914
-913.750447	23.403550	5.135910
-912.465703	22.942321	5.145907
-910.526515	20.731312	5.155904
-908.301649	17.781523	5.165901
-906.501684	19.123055	5.175898
-904.578109	19.958545	5.185894
-902.948603	26.995358	5.195891
-901.074381	18.469922	5.205888
-899.536813	20.846499	5.215885
-897.172044	25.928001	5.225882
-895.370826	24.391122	5.235878
-893.285308	26.689575	5.245875
-891.722952	23.389432	5.255872
-889.685064	17.381347	5.265869
-887.709910	24.686573	5.275866
-886.090550	25.453879	5.285862
-884.197392	22.800282	5.295859
-881.856785	24.642731	5.305856
-880.408404	29.441307	5.315853
-878.401992	27.451666	5.325850
-876.545756	23.536170	5.335846
-874.627541	24.642523	5.345843
-873.077062	25.038771	5.355840
-871.208285	32.762048	5.365837
-868.946406	27.283392	5.375834
-866.866672	29.243344	5.385830
-865.513625	20.029195	5.395827
-863.407783	22.807551	5.405824
-861.588256	12.577850	5.415821
-859.742836	25.425035	5.425818
-857.922917	17.123033	5.435814
-855.822636	16.310429	5.445811
-853.952438	17.385003	5.455808
-851.982431	17.467903	5.465805
-850.313841	26.154709	5.475802
-848.656824	6.007478	5.485798
-846.897876	18.282743	5.495795
-844.600521	20.769994	5.505792
-842.973186	18.844136	5.515789
-840.809102	16.988786	5.525786
-838.937200	14.599131	5.535782
-837.106761	18.899324	5.545779
-835.265219	21.071050	5.555776
-833.448171	21.317353	5.565773
-831.358221	22.119994	5.575770
-829.706660	21.606491	5.585766
-827.892140	11.148683	5.595763
-825.896615	19.593786	5.605760
-824.017230	14.751010	5.615757
-822.558534	19.587445	5.625754
-820.436834	20.192402	5.635750
-818.207202	17.317718	5.645747
-816.626633	20.810032	5.655744
-814.559091	21.788363	5.665741
-812.624359	9.070980	5.675738
-811.084519	26.743037	5.685734
-808.937690	28.652847	5.695731
-807.188866	19.244423	5.705728
-805.099176	18.657751	5.715725
-803.365350	18.617400	5.725722
-801.782914	19.562759	5.735718
-799.574250	17.198250	5.745715
-797.608553	17.768167	5.755712
-795.941458	15.155507	5.765709
-794.030483	21.762178	5.775706
-792.363693	19.681637	5.785702
-790.369388	18.614468	5.795699
-788.296433	16.928456	5.805696
-786.502936	14.789777	5.815693
-784.647284	8.919845	5.825690
-782.971924	23.365222	5.835686
-780.818956	14.253781	5.845683
-779.025184	16.745796	5.855680
-777.194200	20.318108	5.865677
-775.026481	8.555025	5.875674
-773.304241	24.251254	5.885670
-771.616504	21.393748	5.895667
-769.858986	19.142417	5.905664
-767.829641	15.619309	5.915661
-765.587934	19.072309	5.925658
-763.963976	23.806588	5.935654
-762.258621	21.326773	5.945651
-760.430436	18.509983	5.955648
-758.479122	22.244647	5.965645
-756.375644	20.318537	5.975642
-754.635475	27.568290	5.985638
-752.737532	16.986676	5.995635
-750.719388	18.628176	6.005632
-748.721726	19.579841	6.015629
-746.969872	19.059840	6.025626
-745.323274	21.629083	6.035622
-743.864671	19.431856	6.045619
-741.667493	22.558861	6.055616
-739.369739	12.680683	6.065613
-737.760019	28.499133	6.075610
-735.869300	19.467525	6.085606
-733.893348	29.224707	6.095603
-732.120906	23.489675	6.105600
-730.266360	19.280894	6.115597
-728.443303	26.157447	6.125594
-726.394027	25.218905	6.135590
-724.674153	14.953116	6.145587
-722.636627	18.464047	6.155584
-720.689540	18.487566	6.165581
-718.843328	24.714680	6.175578
-717.341876	26.509824	6.185574
-715.331786	17.986490	6.195571
-713.409193	14.952558	6.205568
-711.495871	27.231701	6.215565
-709.461264	15.928853	6.225562
-707.479988	18.245710	6.235558
-706.004897	18.620959	6.245555
-704.055185	18.721435	6.255552
-702.228343	19.214152	6.265549
-699.844601	18.277449	6.275546
-698.572078	24.964119	6.285542
-696.493315	27.761167	6.295539
-694.470857	21.780962	6.305536
-692.402960	21.581529	6.315533
-691.049635	25.770199	6.325530
-689.119231	20.017852	6.335526
-687.090097	23.662780	6.345523
-685.150798	21.641394	6.355520
-683.214003	22.236550	6.365517
-681.366579	20.120907	6.375514
-679.634976	19.905751	6.385510
-677.788103	18.702769	6.395507
-675.803930	33.277317	6.405504
-673.939465	21.401716	6.415501
-672.256371	27.583886	6.425498
-670.285582	24.660698	6.435494
-668.075894	21.775127	6.445491
-666.341654	30.066357	6.455488
-664.626210	28.964905	6.465485
-662.858481	26.944109	6.475482
-660.805673	35.713360	6.485478
-658.658145	33.093500	6.495475
-657.435918	27.339064	6.505472
-655.091205	19.550153	6.515469
-653.107941	26.257499	6.525466
-651.386876	19.356074	6.535462
-649.420290	31.852545	6.545459
-647.672952	24.356435	6.555456
-645.707013	18.350565	6.565453
-644.056704	14.847066	6.575450
-642.127408	21.638826	6.585446
-640.102718	20.925324	6.595443
-638.668326	25.443683	6.605440
-636.642163	26.253532	6.615437
-634.504074	23.875186	6.625434
-632.287823	25.442511	6.635430
-630.621558	21.265462	6.645427
-629.088318	19.293205	6.655424
-627.057813	23.539506	6.665421
-625.082248	18.111550	6.675418
-623.398653	25.741475	6.685414
-621.484983	21.210718	6.695411
-619.397513	21.292413	6.705408
-617.765866	23.336805	6.715405
-615.586004	36.441829	6.725402
-614.068476	24.294868	6.735398
-612.051591	17.734606	6.745395
-610.187414	18.717187	6.755392
-608.338895	27.561748	6.765389
-606.034755	17.774233	6.775386
-604.794447	23.316710	6.785382
-602.683292	33.194516	6.795379
-600.673674	17.118158	6.805376
-598.722535	17.509000	6.815373
-596.907968	16.871730	6.825370
-595.116224	19.043710	6.835366
-593.245434	22.617707	6.845363
-591.398602	14.815238	6.855360
-589.896185	21.103694	6.865357
-587.334790	17.266810	6.875354
-585.857524	25.027612	6.885350
-584.003858	24.163068	6.895347
-582.140399	15.843246	6.905344
-580.044791	14.362202	6.915341
-578.080771	21.410560	6.925338
-576.337231	19.925761	6.935334
-574.494714	23.925841	6.945331
-572.726941	21.287776	6.955328
-570.626922	20.699659	6.965325
-568.872848	18.093783	6.975322
-566.905301	24.956866	6.985318
-565.237059	19.080709	6.995315
-563.305339	15.447054	7.005312
-561.278467	17.000488	7.015309
-559.460388	15.521163	7.025306
-557.886352	15.452834	7.035302
-555.853249	24.830024	7.045299
-553.769085	20.535752	7.055296
-551.978287	20.164400	7.065293
-550.146595	15.397335	7.075290
-548.320788	23.257219	7.085286
-546.292046	19.890692	7.095283
-544.416747	26.288561	7.105280
-542.729395	21.279308	7.115277
-540.814235	16.323667	7.125274
-538.892563	21.130552	7.135270
-536.679049	22.022660	7.145267
-534.855879	24.379129	7.155264
-533.215018	19.001544	7.165261
-531.604336	15.313408	7.175258
-529.729674	21.780858	7.185254
-527.611559	19.330011	7.195251
-525.545272	15.888037	7.205248
-523.932313	12.568991	7.215245
-521.988752	22.547843	7.225242
-520.003289	8.259500	7.235238
-518.190132	20.025905	7.245235
-516.296181	18.379767	7.255232
-514.375310	16.389880	7.265229
-512.729183	23.020153	7.275226
-510.596126	16.724029	7.285222
-508.875464	17.017552	7.295219
-506.900654	19.176152	7.305216
-505.214731	25.653243	7.315213
-503.374656	18.994995	7.325210
-501.424951	34.831983	7.335206
-499.388906	27.649837	7.345203
-497.371196	23.806722	7.355200
-495.483255	21.937363	7.365197
-493.732238	30.424991	7.375194
-492.033328	24.834488	7.385190
-490.304143	23.614131	7.395187
-487.834825	17.815341	7.405184
-486.303754	26.627026	7.415181
-484.561640	21.853787	7.425178
-482.611468	25.175214	7.435174
-480.744043	17.982123	7.445171
-478.910176	24.934523	7.455168
-476.942004	21.932965	7.465165
-474.857482	12.921117	7.475162
-473.345228	19.863304	7.485158
-471.444575	17.639852	7.495155
-469.265511	16.161365	7.505152
-467.329481	6.971146	7.515149
-465.665366	24.011057	7.525146
-463.694557	14.872121	7.535142
-462.000518	19.715422	7.545139
-460.118317	21.208369	7.555136
-458.166685	11.859357	7.565133
-455.923548	18.981666	7.575130
-454.225784	18.336315	7.585126
-453.126205	15.190867	7.595123
-450.998040	19.033335	7.605120
-448.581613	25.922733	7.615117
-446.860229	15.361627	7.625114
-445.086761	22.691570	7.635110
-443.090090	25.072509	7.645107
-441.243376	23.179778	7.655104
-439.186302	21.108204	7.665101
-437.615855	15.246166	7.675098
-435.825181	27.328853	7.685094
-433.475279	25.190000	7.695091
-432.038785	22.701242	7.705088
-429.749353	19.179507	7.715085
-427.895083	23.282034	7.725082
-426.319356	21.880976	7.735078
-424.686139	27.739746	7.745075
-422.731049	26.218119	7.755072
-420.534256	21.186019	7.765069
-418.736106	18.628471	7.775066
-416.915400	21.141733	7.785062
-414.801254	20.180468	7.795059
-413.110597	15.200772	7.805056
-411.310422	25.660488	7.815053
-409.264094	14.865954	7.825050
-407.569116	21.829537	7.835046
-405.561089	18.916404	7.845043
-403.758049	22.747675	7.855040
-401.523757	15.306603	7.865037
-399.851702	20.395025	7.875034
-398.413919	21.423750	7.885030
-396.605730	26.182566	7.895027
-394.397840	19.719862	7.905024
-392.293100	22.543034	7.915021
-390.523638	24.835565	7.925018
-388.669879	20.767677	7.935014
-387.061428	18.309909	7.945011
-385.126866	23.021717	7.955008
-383.026120	16.195628	7.965005
-381.268485	15.764966	7.975002
-379.492879	16.332424	7.984998
-377.477618	9.251587	7.994995
-375.593564	18.398547	8.004992
-373.638992	16.341815	8.014989
-371.747329	9.141776	8.024986
-370.013326	15.334994	8.034982
-368.002905	13.360923	8.044979
-366.224125	19.202809	8.054976
-364.426153	13.162395	8.064973
-362.516618	19.539163	8.074970
-360.567514	12.585733	8.084966
-358.481740	10.662794	8.094963
-357.036181	10.419331	8.104960
-354.864725	12.379308	8.114957
-352.930080	4.215642	8.124954
-351.275731	10.121609	8.134950
-349.430360	18.393772	8.144947
-347.199418	5.196813	8.154944
-345.904536	4.197461	8.164941
-343.659621	22.638347	8.174938
-341.988668	14.600458	8.184934
-340.096160	20.308954	8.194931
-337.960306	22.700920	8.204928
-336.273171	19.681184	8.214925
-334.201506	17.664208	8.224922
-332.424608	22.162824	8.234918
-330.526282	14.366523	8.244915
-328.658589	16.242392	8.254912
-326.940392	12.935092	8.264909
-324.858023	19.450081	8.274906
-322.952376	11.764716	8.284902
-321.148966	10.660518	8.294899
-319.232328	8.475683	8.304896
-317.495833	10.741953	8.314893
-315.737914	16.143553	8.324890
-313.998304	14.987968	8.334886
-311.754935	10.867420	8.344883
-309.726892	19.132562	8.354880
-307.942580	11.682878	8.364877
-306.199333	5.176010	8.374874
-304.433740	11.447915	8.384870
-302.523573	13.312288	8.394867
-300.493763	14.214993	8.404864
-298.530591	11.893281	8.414861
-296.984460	14.812019	8.424858
-294.860577	13.123035	8.434854
-292.731064	21.353053	8.444851
-291.372180	17.419487	8.454848
-289.454856	19.770594	8.464845
-287.599085	11.177484	8.474842
-285.469269	15.450867	8.484838
-283.329368	13.083590	8.494835
-281.829925	12.200032	8.504832
-280.004890	13.545941	8.514829
-278.151799	19.031848	8.524826
-276.150052	11.519060	8.534822
-274.503436	13.466572	8.544819
-272.321542	16.440159	8.554816
-270.457066	18.335534	8.564813
-268.683540	13.330075	8.574810
-266.411432	12.244260	8.584807
-265.163817	19.075685	8.594803
-263.011163	21.202949	8.604800
-261.240012	15.043735	8.614797
-259.288582	14.241200	8.624794
-257.204805	11.693442	8.634791
-255.941821	22.362178	8.644787
-253.665018	14.503946	8.654784
-251.661269	16.800239	8.664781
-249.664344	7.399941	8.674778
-248.055867	16.117342	8.684775
-246.178738	22.684109	8.694771
-244.243045	16.624953	8.704768
-242.381951	10.764011	8.714765
-240.360203	8.139330	8.724762
-238.501141	23.844201	8.734759
-236.580913	11.944202	8.744755
-234.844661	7.677301	8.754752
-232.976655	9.952645	8.764749
-231.027440	4.563934	8.774746
-229.280073	13.016039	8.784743
-227.444387	12.846173	8.794739
-225.358105	13.416266	8.804736
-223.528558	14.043123	8.814733
-221.737543	11.736314	8.824730
-219.980291	11.537921	8.834727
-218.207244	15.669369	8.844723
-215.928952	13.921076	8.854720
-214.213597	11.054805	8.864717
-212.335659	17.141499	8.874714
-210.421460	17.416983	8.884711
-208.914110	4.607168	8.894707
-206.976375	6.115136	8.904704
-204.893287	14.477372	8.914701
-202.903060	-3.319710	8.924698
-201.053623	8.153828	8.934695
-199.250676	6.647187	8.944691
-197.424980	5.076921	8.954688
-195.583881	-1.380754	8.964685
-193.550902	13.222778	8.974682
-191.875073	10.552291	8.984679
-189.740211	20.620913	8.994675
-188.147216	15.877986	9.004672
-185.995963	7.341999	9.014669
-183.898554	8.022451	9.024666
-182.567793	3.011923	9.034663
-180.363023	9.273841	9.044659
-178.773395	12.263082	9.054656
-177.009762	14.327771	9.064653
-174.471464	13.771109	9.074650
-173.155065	18.392276	9.084647
-170.922232	10.612181	9.094643
-169.374780	17.526862	9.104640
-167.271735	23.579256	9.114637
-165.328679	15.513844	9.124634
-163.713934	22.466738	9.134631
-161.714268	22.013404	9.144627
-159.876665	14.252174	9.154624
-157.950978	11.799193	9.164621
-155.753689	17.754458	9.174618
-154.649764	19.243945	9.184615
-152.598558	14.576339	9.194611
-150.608906	17.275996	9.204608
-148.382337	13.434571	9.214605
-146.523939	19.879681	9.224602
-144.928641	2.628770	9.234599
-142.780884	13.978981	9.244595
-141.358432	24.164482	9.254592
-139.067734	25.311472	9.264589
-137.016206	13.160075	9.274586
-135.577945	26.502338	9.284583
-133.753646	17.355436	9.294579
-131.819093	18.019290	9.304576
-129.544750	13.503983	9.314573
-127.937159	23.375761	9.324570
-126.012842	22.489242	9.334567
-124.180253	23.088849	9.344563
-122.259320	18.817817	9.354560
-120.681206	23.138329	9.364557
-118.685277	24.438151	9.374554
-116.427526	24.531011	9.384551
-114.989613	26.467727	9.394547
-113.158559	22.259985	9.404544
-110.941034	10.985228	9.414541
-109.066532	24.548417	9.424538
-107.148527	17.682233	9.434535
-105.524702	18.117804	9.444531
-103.625413	23.721216	9.454528
-101.716735	15.140313	9.464525
-99.886928	21.702124	9.474522
-98.067134	16.452570	9.484519
-96.042481	25.117906	9.494515
-94.068853	19.018072	9.504512
-92.114179	24.484772	9.514509
-90.551777	20.002557	9.524506
-88.415177	17.686497	9.534503
-86.569194	22.134814	9.544499
-84.712195	19.757579	9.554496
-83.292290	26.170075	9.564493
-81.111464	24.589025	9.574490
-79.022414	25.760347	9.584487
-77.236912	23.771870	9.594483
-75.353324	15.708114	9.604480
-73.850844	17.554032	9.614477
-71.627662	19.605487	9.624474
-69.978938	24.757878	9.634471
-68.042639	27.900303	9.644467
-65.922980	22.326634	9.654464
-63.977026	19.532617	9.664461
-61.926861	24.748860	9.674458
-60.365309	23.331351	9.684455
-58.725769	27.871042	9.694451
-56.870999	23.331156	9.704448
-55.000931	30.053943	9.714445
-52.445675	22.159354	9.724442
-50.967725	22.253517	9.734439
-49.023007	21.670102	9.744435
-47.378764	22.988192	9.754432
-45.587342	22.514491	9.764429
-43.435361	25.044671	9.774426
-41.614451	27.899227	9.784423
-39.794597	20.103013	9.794419
-37.820187	20.252194	9.804416
-36.061552	21.730455	9.814413
-33.981093	13.663745	9.824410
-32.250852	21.375108	9.834407
-30.452764	28.322542	9.844403
-28.562453	24.612219	9.854400
-26.522756	25.643048	9.864397
-24.787507	27.145573	9.874394
-22.813875	22.672009	9.884391
-21.109326	20.375977	9.894387
-19.163821	24.191144	9.904384
-17.183748	21.146998	9.914381
-15.205103	19.085129	9.924378
-13.504960	21.156911	9.934375
-11.812907	20.770133	9.944371
-9.731210	20.016488	9.954368
-7.595270	21.936664	9.964365
-5.747494	19.259398	9.974362
-4.279161	18.747266	9.984359
-3.053427	49.044120	9.994355
-1.901366	82.816808	10.004352
-0.717134	145.300840	10.014349
0.000000	210.106534	10.019354
0.607087	247.565671	10.024359
1.497901	292.179609	10.029363
1.965136	329.164552	10.034368
2.027841	362.798608	10.039373
2.500028	393.511711	10.044378
3.144514	417.293828	10.049383
3.158863	450.536851	10.054387
3.426799	451.894359	10.059392
3.663854	471.805656	10.064397
3.801329	476.862843	10.069402
3.900125	501.238314	10.074407
4.091544	503.133134	10.079411
3.999908	506.672064	10.084416
3.932953	515.782933	10.089421
4.269279	524.011080	10.094426
4.690582	534.849623	10.099431
4.429387	559.582218	10.104435
4.704803	555.748991	10.109440
4.561689	561.167915	10.114445
4.628445	555.519850	10.119450
4.627063	559.809190	10.124455
4.264335	572.644583	10.129459
4.477615	564.743416	10.134464
4.375804	562.827933	10.139469
4.585144	574.400454	10.144474
4.572544	595.685793	10.149479
4.761816	609.428198	10.154483
4.886141	612.312988	10.159488
5.077270	613.420997	10.164493
5.283907	609.448920	10.169498
5.163813	608.223874	10.174503
5.141888	615.402231	10.179507
5.467760	611.239254	10.184512
5.194817	615.712268	10.189517
5.226990	610.900722	10.194522
5.179435	627.446797	10.199527
5.333125	628.808352	10.204531
5.711353	626.346380	10.209536
5.583448	634.500405	10.214541
5.689562	633.059511	10.219546
5.549426	643.785840	10.224551
5.834502	660.923853	10.229555
6.191856	656.941917	10.234560
5.669002	644.752250	10.239565
5.817711	646.295944	10.244570
5.931957	638.672299	10.249575
5.849086	648.571086	10.254579
5.818958	641.169156	10.259584
5.980463	656.472436	10.264589
6.091139	675.128456	10.269594
6.223028	666.554261	10.274599
6.122147	679.187140	10.279603
6.361201	667.842576	10.284608
6.231745	688.167431	10.289613
6.491782	681.860881	10.294618
6.456599	678.433541	10.299623
6.176110	688.198299	10.304627
6.494818	689.982959	10.309632
6.146204	688.791200	10.314637
6.679110	684.005419	10.319642
6.532817	686.871887	10.324647
6.263388	692.154893	10.329651
6.727026	689.195178	10.334656
6.127978	699.143212	10.339661
6.460895	696.585957	10.344666
6.432996	687.034323	10.349671
6.301309	697.234234	10.354675
6.726193	711.251385	10.359680
6.637795	720.930335	10.364685
6.584196	726.991039	10.369690
6.597233	731.530436	10.374695
6.606074	727.695528	10.379699
7.163812	729.484645	10.384704
6.928873	742.665649	10.389709
6.887563	737.473131	10.394714
7.255770	733.013215	10.399719
7.155400	742.414977	10.404723
7.169999	738.449840	10.409728
7.020268	751.435917	10.414733
7.494282	758.539976	10.419738
7.486556	766.302755	10.424743
7.083085	778.245985	10.429747
7.759972	776.297736	10.434752
7.601651	780.199021	10.439757
7.475544	790.536876	10.444762
7.761973	772.482775	10.449767
7.675833	773.828980	10.454771
7.753133	773.078627	10.459776
7.568255	791.436591	10.464781
7.579561	783.867134	10.469786
7.491244	786.055761	10.474791
7.509132	783.245968	10.479795
7.593625	782.645852	10.484800
7.608699	797.603638	10.489805
7.846331	804.377999	10.494810
8.538350	804.062599	10.499815
8.075506	817.565443	10.504819
8.191757	814.273187	10.509824
8.251155	822.231867	10.514829
8.541816	810.044769	10.519834
8.630666	790.568238	10.524839
8.052277	796.209635	10.529843
8.347088	799.833654	10.534848
8.614707	809.055343	10.539853
8.339628	824.119358	10.544858
8.466972	811.387462	10.549863
8.203821	824.339656	10.554867
8.449503	826.284210	10.559872
8.426968	827.019469	10.564877
8.446388	832.937686	10.569882
8.515487	833.563715	10.574887
8.558487	836.903059	10.579891
8.694492	835.602455	10.584896
8.558802	835.904761	10.589901
8.755749	840.482668	10.594906
9.075342	847.075246	10.599911
8.937235	848.584285	10.604915
9.214789	852.575338	10.609920
9.036798	856.812512	10.614925
9.020553	862.749045	10.619930
9.328993	865.369558	10.624935
8.887723	874.417353	10.629939
9.315187	874.716571	10.634944
9.231095	874.185916	10.639949
9.471276	873.419041	10.644954
9.191930	867.936441	10.649959
9.011265	884.817848	10.654963
9.266319	862.742743	10.659968
9.116108	877.679666	10.664973
9.084825	889.213547	10.669978
9.579576	878.414654	10.674983
9.309899	885.292043	10.679987
9.736239	893.435084	10.684992
9.838626	901.330181	10.689997
9.760037	901.054110	10.695002
9.970383	898.839640	10.700007
9.711052	906.000813	10.705011
10.056377	896.935131	10.710016
9.738126	911.110425	10.715021
9.610059	908.456349	10.720026
10.166962	899.252843	10.725031
9.880391	905.943705	10.730035
9.801965	907.876887	10.735040
10.230262	911.829723	10.740045
9.766116	907.652318	10.745050
9.936679	912.921998	10.750055
9.918028	915.137379	10.755059
10.405091	924.587490	10.760064
10.720753	942.052115	10.765069
10.490802	941.527374	10.770074
10.595280	945.027247	10.775079
10.470598	949.519293	10.780083
10.995269	935.137520	10.785088
10.606421	926.136878	10.790093
10.625515	922.727631	10.795098
10.722077	917.349058	10.800103
10.572684	935.955431	10.805107
10.897218	946.117444	10.810112
10.824162	944.824944	10.815117
10.861482	939.583543	10.820122
11.349701	939.918804	10.825127
10.799663	938.191453	10.830131
11.097549	939.621502	10.835136
11.214735	939.826709	10.840141
11.164461	938.391805	10.845146
11.048021	951.267096	10.850151
10.820400	952.121802	10.855155
11.203907	938.002236	10.860160
11.227226	945.380119	10.865165
11.166006	947.023560	10.870170
11.557150	945.888832	10.875175
11.233795	948.149663	10.880179
11.503313	939.769397	10.885184
11.532543	940.647790	10.890189
11.530927	958.795390	10.895194
11.789697	949.513248	10.900199
11.473102	946.441384	10.905203
11.699573	949.264219	10.910208
11.453705	947.070466	10.915213
11.535060	950.001600	10.920218
11.982078	940.331476	10.925223
11.861972	950.165445	10.930227
11.906771	940.958436	10.935232
12.086949	943.943193	10.940237
11.803611	944.500860	10.945242
11.721933	950.130901	10.950247
11.481313	960.857721	10.955251
11.930845	962.110623	10.960256
12.217296	987.008910	10.965261
12.001691	978.248683	10.970266
12.156276	980.721871	10.975271
12.268266	981.435681	10.980275
12.480798	989.420491	10.985280
12.521080	994.423976	10.990285
12.791760	983.059930	10.995290
12.706794	980.167156	11.000295
12.509340	994.241265	11.005299
12.596012	981.750670	11.010304
12.408082	992.445456	11.015309
12.321272	989.890439	11.020314
12.734755	985.607729	11.025319
12.577782	993.596281	11.030323
12.495798	988.640393	11.035328
12.681786	996.326668	11.040333
12.669261	978.211184	11.045338
12.863518	981.964826	11.050343
12.547017	997.161782	11.055347
12.954819	986.755142	11.060352
12.993106	993.555079	11.065357
12.657689	989.529005	11.070362
12.713939	1008.400714	11.075367
13.141149	1017.698008	11.080371
13.323414	1027.345033	11.085376
12.927907	1017.372421	11.090381
13.271761	1028.964853	11.095386
13.351782	1030.235695	11.100391
13.303134	1023.878883	11.105395
13.545249	1015.282172	11.110400
13.676877	1032.897683	11.115405
13.079864	1027.435725	11.120410
13.385745	1017.988331	11.125415
13.110442	1029.693707	11.130419
12.961566	1027.869246	11.135424
13.445032	1042.785697	11.140429
14.142078	1047.178252	11.145434
14.137991	1040.833248	11.150439
14.078843	1062.662859	11.155443
14.210209	1054.894339	11.160448
14.381519	1039.397152	11.165453
13.936898	1027.713496	11.170458
14.079491	1013.982362	11.175463
14.027650	1022.286897	11.180467
14.081260	1020.603606	11.185472
13.748784	1018.256499	11.190477
14.117951	1019.738265	11.195482
14.448374	1018.535947	11.200487
14.185160	1027.883441	11.205491
14.189127	1027.750318	11.210496
14.480327	1027.044684	11.215501
14.115593	1030.602067	11.220506
14.489091	1041.483310	11.225511
14.463599	1050.381322	11.230515
14.726452	1038.603743	11.235520
14.869603	1051.040330	11.240525
14.683628	1035.440860	11.245530
14.905255	1012.462538	11.250535
14.632702	1011.402121	11.255539
14.536439	1017.029784	11.260544
14.864117	1017.532579	11.265549
15.088712	1033.029622	11.270554
15.008963	1019.773911	11.275559
14.693901	1021.732235	11.280563
14.800506	1029.380726	11.285568
14.936604	1043.909460	11.290573
14.862694	1051.272941	11.295578
15.116136	1052.528742	11.300583
14.971892	1053.504196	11.305587
15.001248	1055.420207	11.310592
15.056298	1057.694818	11.315597
14.865626	1052.893437	11.320602
15.327285	1045.613136	11.325607
15.249272	1053.052966	11.330611
15.336121	1055.030771	11.335616
15.371242	1056.805514	11.340621
15.372389	1049.896702	11.345626
15.705024	1044.119309	11.350631
15.283896	1063.133459	11.355635
15.372990	1056.797241	11.360640
15.615144	1064.108743	11.365645
15.649857	1088.602657	11.370650
15.915163	1089.072824	11.375655
15.755623	1088.667735	11.380659
16.154858	1082.662085	11.385664
16.168220	1076.888292	11.390669
15.918656	1074.143177	11.395674
15.993007	1058.224619	11.400679
16.073553	1072.207155	11.405683
16.167640	1068.129903	11.410688
16.252043	1051.714587	11.415693
15.794849	1059.069818	11.420698
16.305767	1064.331001	11.425703
16.254253	1073.367217	11.430707
16.250781	1069.772301	11.435712
16.460478	1077.150487	11.440717
16.336860	1082.478187	11.445722
16.541461	1082.844496	11.450727
16.300209	1072.415158	11.455731
16.337094	1083.796397	11.460736
16.467935	1082.964950	11.465741
16.467969	1090.020191	11.470746
16.482001	1078.320112	11.475751
16.362989	1091.402519	11.480755
16.633377	1080.492605	11.485760
16.828229	1079.669871	11.490765
16.940944	1087.886698	11.495770
17.110412	1078.869452	11.500775
16.865617	1077.489213	11.505779
16.887733	1079.325958	11.510784
16.939251	1080.814239	11.515789
16.797040	1084.843922	11.520794
16.965258	1089.998923	11.525799
16.707696	1092.003278	11.530803
17.068956	1085.833373	11.535808
16.922765	1095.893952	11.540813
17.160677	1112.092276	11.545818
17.626891	1108.971220	11.550823
17.491188	1110.508287	11.555827
17.557472	1112.951426	11.560832
17.443152	1090.684151	11.565837
17.236226	1082.264674	11.570842
17.501639	1088.717772	11.575847
17.309664	1121.492195	11.580851
17.529363	1106.353072	11.585856
17.909601	1113.177375	11.590861
17.640248	1113.398502	11.595866
17.774519	1112.282655	11.600871
17.534623	1114.528622	11.605875
17.609684	1115.951651	11.610880
17.928097	1114.543083	11.615885
18.098197	1113.166054	11.620890
17.877831	1114.059035	11.625895
17.810456	1117.657322	11.630899
17.884707	1116.625164	11.635904
18.174438	1100.968675	11.640909
17.931851	1119.569647	11.645914
18.100128	1112.358182	11.650919
18.143614	1117.422700	11.655923
18.159642	1117.432732	11.660928
18.276640	1109.338468	11.665933
18.086719	1115.670235	11.670938
18.257639	1105.682914	11.675943
18.313299	1121.769969	11.680947
18.312429	1127.737275	11.685952
18.785881	1139.441591	11.690957
18.535521	1141.577268	11.695962
18.841290	1131.090605	11.700967
18.371367	1130.708209	11.705971
18.525390	1137.727875	11.710976
18.843910	1137.388464	11.715981
18.688526	1134.363387	11.720986
18.920090	1129.489907	11.725991
18.713742	1144.748295	11.730995
19.270582	1139.384539	11.736000
19.420523	1137.857759	11.741005
19.142600	1121.591615	11.746010
19.113376	1109.130433	11.751015
18.951480	1103.693664	11.756019
18.925666	1119.216546	11.761024
19.313966	1133.476488	11.766029
19.162633	1135.362981	11.771034
19.303320	1136.807084	11.776039
19.138662	1142.921944	11.781043
18.828868	1144.250237	11.786048
19.356311	1139.227061	11.791053
19.017408	1145.369713	11.796058
19.175905	1141.928720	11.801063
19.113146	1145.900016	11.806067
19.232781	1144.862194	11.811072
19.538448	1152.948936	11.816077
19.355117	1164.026315	11.821082
19.881812	1151.544242	11.826087
19.850611	1161.723722	11.831091
20.058350	1165.938888	11.836096
20.240922	1165.313652	11.841101
19.637547	1154.710197	11.846106
19.961738	1150.693994	11.851111
20.042346	1159.677653	11.856115
20.203664	1160.558647	11.861120
19.787866	1159.196212	11.866125
19.996871	1163.948918	11.871130
20.196547	1165.648545	11.876135
20.115715	1166.306385	11.881139
19.907592	1168.290250	11.886144
20.590554	1159.695683	11.891149
20.089819	1167.925239	11.896154
20.374480	1159.958749	11.901159
20.273903	1162.292891	11.906163
20.164194	1162.501173	11.911168
20.343668	1167.797910	11.916173
19.959584	1156.446693	11.921178
20.268100	1150.397138	11.926183
20.260036	1170.949315	11.931187
20.292943	1194.497521	11.936192
20.700610	1186.788943	11.941197
20.315911	1196.010840	11.946202
20.599763	1199.092657	11.951207
20.961179	1200.071052	11.956211
20.830944	1184.721151	11.961216
21.120586	1186.398547	11.966221
20.979333	1193.883229	11.971226
21.496352	1183.793347	11.976231
21.080255	1185.332564	11.981235
21.191190	1187.656630	11.986240
21.461081	1182.426934	11.991245
21.541249	1189.622409	11.996250
21.379672	1189.835810	12.001255
21.388112	1189.064879	12.006259
21.325638	1192.602478	12.011264
21.441896	1185.634241	12.016269
21.488156	1191.407975	12.021274
21.646353	1173.692374	12.026279
21.581326	1190.919972	12.031283
21.132980	1176.246869	12.036288
21.373139	1160.812688	12.041293
21.016948	1179.635284	12.046298
21.248907	1185.220125	12.051303
21.383764	1184.451110	12.056307
21.617118	1190.377932	12.061312
21.882333	1186.095157	12.066317
21.624858	1183.040620	12.071322
21.762274	1153.837051	12.076327
21.761873	1149.273373	12.081331
21.522302	1146.104025	12.086336
21.570734	1147.359415	12.091341
21.500885	1151.019606	12.096346
21.259784	1141.575792	12.101351
21.548772	1151.612734	12.106355
21.668752	1154.966683	12.111360
21.996144	1148.564034	12.116365
21.417130	1162.429500	12.121370
21.757368	1158.663049	12.126375
21.454022	1151.440051	12.131379
21.234917	1134.453303	12.136384
21.425086	1134.597988	12.141389
21.417177	1142.636965	12.146394
21.622957	1136.318372	12.151399
21.580612	1130.230166	12.156403
21.553403	1128.220707	12.161408
21.644346	1114.179171	12.166413
21.272930	1122.916356	12.171418
21.622513	1118.497142	12.176423
21.412937	1127.590141	12.181427
21.314191	1129.603864	12.186432
21.741733	1124.937249	12.191437
21.397701	1119.196785	12.196442
21.559883	1119.998792	12.201447
21.133678	1128.259017	12.206451
21.391601	1123.972692	12.211456
21.384700	1121.889032	12.216461
21.409527	1118.392092	12.221466
21.432628	1124.875969	12.226471
21.528833	1124.961523	12.231475
21.148134	1128.120928	12.236480
21.501227	1134.344021	12.241485
21.657023	1133.771942	12.246490
21.752517	1126.340266	12.251495
21.650962	1135.067534	12.256499
21.697486	1130.617804	12.261504
21.849581	1129.514882	12.266509
21.428055	1125.773738	12.271514
21.466915	1099.785636	12.276519
21.339316	1097.631344	12.281523
21.239412	1100.171949	12.286528
21.296147	1091.303562	12.291533
21.111801	1101.460116	12.296538
21.678878	1111.296560	12.301543
21.504232	1123.944745	12.306547
21.366776	1123.219164	12.311552
21.458752	1106.383108	12.316557
21.105259	1111.294896	12.321562
21.655705	1121.774243	12.326567
21.465328	1121.421378	12.331571
21.313650	1110.321714	12.336576
21.189260	1113.128001	12.341581
21.612624	1120.929449	12.346586
21.773618	1108.799052	12.351591
21.367689	1112.121750	12.356595
21.282197	1107.560618	12.361600
21.651284	1100.600983	12.366605
21.110590	1105.522125	12.371610
21.252748	1107.196226	12.376615
21.489333	1106.999193	12.381619
21.169942	1105.671849	12.386624
21.781777	1105.400776	12.391629
21.421667	1105.603262	12.396634
21.585083	1109.448589	12.401639
21.524896	1110.748108	12.406643
21.198621	1111.255857	12.411648
21.449726	1107.476827	12.416653
21.097039	1098.888199	12.421658
21.385784	1106.837266	12.426663
21.464482	1106.436756	12.431667
21.250168	1105.520008	12.436672
21.394675	1112.228943	12.441677
21.042331	1115.401170	12.446682
21.416660	1129.966112	12.451687
21.437241	1141.496655	12.456691
21.330011	1150.226414	12.461696
21.599486	1134.576273	12.466701
21.307225	1140.027085	12.471706
21.746615	1135.825356	12.476711
21.460561	1125.731131	12.481715
21.212632	1113.126631	12.486720
21.548127	1110.406468	12.491725
21.497044	1112.645976	12.496730
21.790708	1103.320325	12.501735
21.607032	1105.093700	12.506739
21.392189	1119.711599	12.511744
21.307194	1105.802209	12.516749
20.994632	1116.229958	12.521754
21.391522	1119.940281	12.526759
21.297038	1121.636355	12.531763
21.501401	1123.603312	12.536768
21.706990	1108.980523	12.541773
21.192417	1108.701442	12.546778
21.584281	1111.433277	12.551783
21.720907	1112.895372	12.556787
21.554073	1111.251959	12.561792
21.781854	1119.485146	12.566797
21.445498	1118.075351	12.571802
21.683015	1111.556164	12.576807
21.497829	1110.707310	12.581811
21.485215	1114.823564	12.586816
21.861698	1113.848859	12.591821
21.416017	1107.414983	12.596826
21.650035	1092.691482	12.601831
21.446118	1090.754366	12.606835
21.197424	1089.130320	12.611840
21.435723	1086.337354	12.616845
21.013596	1089.646861	12.621850
21.232269	1106.766034	12.626855
21.220296	1108.685491	12.631859
21.427989	1117.885398	12.636864
21.219635	1109.164935	12.641869
21.271999	1116.740122	12.646874
21.630748	1110.710957	12.651879
21.572054	1119.571729	12.656883
21.532863	1123.438335	12.661888
21.668414	1115.478304	12.666893
21.427766	1104.118444	12.671898
21.382331	1094.118329	12.676903
21.442192	1092.790423	12.681907
21.219095	1090.446359	12.686912
21.489957	1096.023385	12.691917
20.974548	1099.469197	12.696922
21.288148	1106.592707	12.701927
21.070618	1119.143649	12.706931
21.375522	1125.937396	12.711936
21.586261	1119.472940	12.716941
21.512802	1131.059473	12.721946
21.387510	1125.408699	12.726951
21.592949	1131.885575	12.731955
21.446100	1125.746230	12.736960
21.609551	1131.993259	12.741965
21.240002	1121.942316	12.746970
21.528563	1114.208618	12.751975
21.094809	1110.578238	12.756979
20.954639	1117.647969	12.761984
21.357123	1121.478825	12.766989
21.440880	1120.779465	12.771994
21.367052	1119.419262	12.776999
21.350282	1127.377643	12.782003
21.231029	1137.134332	12.787008
21.385706	1128.434805	12.792013
21.416335	1137.019567	12.797018
21.276374	1135.177901	12.802023
21.464280	1130.156842	12.807027
21.556528	1141.149250	12.812032
21.905028	1131.004280	12.817037
21.676199	1137.343838	12.822042
21.543379	1120.999358	12.827047
21.526189	1118.543602	12.832051
21.295664	1107.808175	12.837056
21.436575	1092.954444	12.842061
21.292084	1102.888600	12.847066
21.299016	1109.315124	12.852071
21.573272	1103.610097	12.857075
21.364649	1101.435610	12.862080
21.357875	1105.300196	12.867085
21.156359	1105.863741	12.872090
21.500029	1115.314772	12.877095
21.297127	1124.118122	12.882099
21.375054	1131.025343	12.887104
21.354527	1131.168938	12.892109
21.186660	1137.230691	12.897114
21.324551	1138.003457	12.902119
21.561344	1132.580361	12.907123
21.357684	1140.076546	12.912128
21.862609	1139.718444	12.917133
21.681301	1125.625700	12.922138
21.535463	1110.587449	12.927143
21.390620	1103.864321	12.932147
21.382211	1105.294353	12.937152
21.254604	1114.202382	12.942157
21.099877	1117.544942	12.947162
21.378420	1104.116892	12.952167
21.549071	1105.594060	12.957171
21.278131	1108.207677	12.962176
21.408614	1101.787567	12.967181
21.335629	1111.428050	12.972186
21.119799	1118.946665	12.977191
21.336740	1116.590763	12.982195
21.236715	1132.820931	12.987200
21.732922	1129.709280	12.992205
21.526235	1135.652645	12.997210
21.241276	1126.356184	13.002215
21.536343	1132.093367	13.007219
21.246398	1136.490402	13.012224
21.612504	1118.087273	13.017229
21.355836	1118.721115	13.022234
21.056681	1113.746204	13.027239
21.645840	1136.781400	13.032243
21.557839	1136.021123	13.037248
21.688041	1114.064896	13.042253
21.444121	1117.486336	13.047258
21.335261	1117.634557	13.052263
21.715913	1102.975969	13.057267
21.219643	1111.800869	13.062272
21.646230	1111.035792	13.067277
21.711956	1111.873683	13.072282
21.590913	1114.518587	13.077287
21.627815	1106.232096	13.082291
21.457808	1121.673899	13.087296
21.754231	1122.902351	13.092301
21.427851	1113.744969	13.097306
21.380048	1117.154054	13.102311
21.378200	1106.188191	13.107315
21.374281	1116.776450	13.112320
21.424497	1117.783971	13.117325
21.159271	1112.969229	13.122330
21.766056	1114.211259	13.127335
21.541305	1111.916340	13.132339
21.439745	1126.788991	13.137344
21.616698	1116.262959	13.142349
21.603057	1112.112990	13.147354
21.181314	1092.739564	13.152359
21.479537	1081.416780	13.157363
21.108531	1093.217895	13.162368
21.410164	1102.513196	13.167373
21.398863	1112.008224	13.172378
21.612215	1105.267391	13.177383
21.532230	1099.729250	13.182387
21.130222	1093.428763	13.187392
21.391158	1104.220775	13.192397
21.755979	1112.321715	13.197402
21.522213	1101.585232	13.202407
21.576284	1083.246106	13.207411
21.308472	1097.082378	13.212416
21.339225	1083.376899	13.217421
21.452216	1088.725212	13.222426
21.407608	1083.610365	13.227431
21.417010	1072.787813	13.232435
21.238770	1081.060503	13.237440
21.544126	1084.714452	13.242445
21.584760	1090.418081	13.247450
21.413431	1085.761836	13.252455
21.506886	1086.331952	13.257459
21.301804	1088.614941	13.262464
21.197054	1086.220463	13.267469
21.277118	1088.661401	13.272474
21.355735	1085.928596	13.277479
21.434233	1079.691828	13.282483
21.135935	1100.428966	13.287488
21.516011	1081.730342	13.292493
21.644450	1089.457385	13.297498
21.364810	1092.974402	13.302503
21.455966	1087.205544	13.307507
21.361453	1090.172642	13.312512
21.549324	1086.432087	13.317517
21.467531	1089.772469	13.322522
21.453061	1086.879469	13.327527
21.606437	1091.202632	13.332531
21.417967	1095.329582	13.337536
21.491928	1086.144637	13.342541
21.596246	1084.987837	13.347546
21.287711	1102.818716	13.352551
21.583120	1095.758871	13.357555
21.453473	1095.479900	13.362560
21.548772	1092.028497	13.367565
21.299451	1102.405149	13.372570
21.510096	1100.993270	13.377575
21.536170	1085.782547	13.382579
21.270135	1104.294200	13.387584
21.675331	1091.736940	13.392589
21.687169	1079.679241	13.397594
21.693913	1113.402816	13.402599
21.502165	1083.204790	13.407603
21.446401	1108.498490	13.412608
21.288964	1070.517490	13.417613
20.948871	1091.961447	13.422618
21.420493	1095.401224	13.427623
21.529845	1079.251556	13.432627
21.379310	1095.887131	13.437632
21.411306	1086.437643	13.442637
21.313450	1095.698884	13.447642
21.436597	1105.304929	13.452647
21.740379	1095.383157	13.457651
21.367821	1088.661661	13.462656
21.614107	1099.552200	13.467661
21.370290	1057.387167	13.472666
21.153566	1079.767060	13.477671
21.666317	1068.777500	13.482675
21.227552	1067.827165	13.487680
21.501237	1092.454861	13.492685
21.472624	1061.877624	13.497690
21.433562	1076.599907	13.502695
21.425263	1071.723701	13.507699
20.960330	1068.677044	13.512704
21.646318	1092.341699	13.517709
21.130702	1070.315074	13.522714
21.212373	1103.473167	13.527719
21.709465	1095.335636	13.532723
21.369302	1104.607143	13.537728
21.644879	1085.851063	13.542733
21.250579	1083.832349	13.547738
21.066629	1074.970819	13.552743
21.449368	1093.984534	13.557747
21.592589	1097.732155	13.562752
21.672863	1090.031689	13.567757
21.580391	1077.629507	13.572762
21.303191	1065.171643	13.577767
21.605028	1059.424387	13.582771
20.851301	1091.216012	13.587776
21.443890	1068.534827	13.592781
21.331123	1077.058846	13.597786
20.978172	1093.428657	13.602791
21.502929	1097.399278	13.607795
21.169003	1105.815083	13.612800
21.364273	1108.053147	13.617805
21.450721	1111.872904	13.622810
21.852025	1099.074984	13.627815
22.074650	1110.209002	13.632819
21.295200	1080.289217	13.637824
21.573617	1078.101711	13.642829
21.215112	1083.241369	13.647834
21.192507	1068.117276	13.652839
21.377330	1070.221382	13.657843
20.863919	1093.970098	13.662848
21.312041	1087.586067	13.667853
21.125682	1095.882137	13.672858
21.353211	1120.457318	13.677863
21.204006	1095.786012	13.682867
21.421306	1126.038281	13.687872
21.066286	1095.200795	13.692877
21.299578	1122.094755	13.697882
21.175534	1101.047999	13.702887
21.036118	1119.254048	13.707891
21.314552	1107.218462	13.712896
21.351288	1116.373095	13.717901
21.729048	1079.082575	13.722906
21.225608	1131.922929	13.727911
21.399907	1100.860662	13.732915
21.427515	1127.528816	13.737920
21.478785	1107.294606	13.742925
21.370298	1116.701059	13.747930
21.588220	1114.086379	13.752935
21.390898	1107.067267	13.757939
21.517290	1095.795531	13.762944
21.657670	1116.125260	13.767949
21.577262	1112.455871	13.772954
21.134233	1122.877624	13.777959
21.641817	1112.350903	13.782963
21.510333	1100.120504	13.787968
21.557854	1110.123389	13.792973
21.548053	1106.294508	13.797978
21.547500	1113.010809	13.802983
21.632852	1108.668434	13.807987
21.648539	1105.512000	13.812992
21.427797	1099.598916	13.817997
21.711609	1089.238788	13.823002
21.392490	1081.359175	13.828007
21.231717	1084.038795	13.833011
21.442337	1103.538867	13.838016
21.314043	1085.247747	13.843021
21.243782	1067.431517	13.848026
21.480602	1095.119645	13.853031
21.405341	1075.057049	13.858035
21.226039	1078.799333	13.863040
21.359446	1083.909422	13.868045
21.674706	1083.608379	13.873050
21.131834	1085.689776	13.878055
21.691288	1084.976049	13.883059
21.117753	1091.769533	13.888064
21.621104	1086.426943	13.893069
21.727259	1080.032800	13.898074
21.547616	1084.290803	13.903079
21.951377	1093.555618	13.908083
21.431028	1088.521376	13.913088
21.395359	1088.279456	13.918093
21.779494	1074.482933	13.923098
21.488567	1097.557507	13.928103
21.586413	1095.155947	13.933107
21.495703	1088.678081	13.938112
21.671115	1081.714651	13.943117
21.656683	1092.269876	13.948122
21.431558	1065.986470	13.953127
21.685312	1058.193698	13.958131
21.315969	1066.247700	13.963136
21.386552	1048.673957	13.968141
21.009554	1051.137323	13.973146
21.160450	1060.445600	13.978151
21.441532	1078.776921	13.983155
21.521142	1088.044546	13.988160
21.399460	1087.975616	13.993165
21.354778	1091.568700	13.998170
21.252751	1107.149456	14.003175
21.826410	1080.000613	14.008179
21.135525	1091.472699	14.013184
21.154674	1086.754536	14.018189
21.532730	1087.790282	14.023207
21.113250	1093.609354	14.028224
21.588674	1091.907094	14.033242
21.267964	1109.733884	14.038259
21.687739	1082.124933	14.043277
21.119811	1088.746277	14.048295
21.232787	1096.114701	14.053312
21.512457	1094.630839	14.058330
21.090704	1091.648170	14.063347
21.213972	1098.118384	14.068365
21.111821	1097.094943	14.073383
20.794007	1101.963484	14.078400
21.211474	1094.994864	14.083418
21.085727	1126.048798	14.088435
21.414786	1130.564083	14.093453
21.413023	1119.501910	14.098471
21.346165	1138.486822	14.103488
21.941260	1128.148948	14.108506
21.610496	1141.612496	14.113523
21.694118	1130.997566	14.118541
21.878655	1126.692878	14.123559
21.868598	1125.749123	14.128576
22.126943	1127.186448	14.133594
21.543427	1128.028200	14.138611
21.953341	1125.159832	14.143629
22.065051	1129.549342	14.148647
22.054826	1138.656651	14.153664
22.068361	1132.582945	14.158682
21.820457	1129.500185	14.163699
21.961842	1130.567650	14.168717
21.974785	1130.290295	14.173735
21.930996	1127.793144	14.178752
21.744739	1131.731559	14.183770
21.552687	1126.079158	14.188787
21.862706	1137.400413	14.193805
21.987571	1132.880311	14.198823
21.663847	1138.127310	14.203840
22.248583	1142.262068	14.208858
22.152396	1138.324600	14.213875
21.801518	1132.051053	14.218893
22.225782	1142.957712	14.223911
22.059363	1169.499189	14.228928
22.094934	1164.331112	14.233946
21.931194	1168.443687	14.238963
22.099150	1170.892674	14.243981
21.959753	1167.514190	14.248999
21.779209	1170.144594	14.254016
22.018545	1172.215703	14.259034
21.996919	1175.327247	14.264051
21.942339	1170.809013	14.269069
21.991726	1165.527054	14.274087
22.273041	1186.048310	14.279104
22.602552	1181.311521	14.284122
22.563883	1180.852071	14.289139
22.285106	1168.209197	14.294157
22.190728	1160.304491	14.299175
22.285337	1180.806756	14.304192
22.132112	1182.460730	14.309210
22.388581	1203.885694	14.314227
22.415977	1207.429850	14.319245
22.584549	1194.248443	14.324263
22.579726	1204.968767	14.329280
22.684007	1205.919466	14.334298
22.599665	1212.202631	14.339315
22.571029	1207.563850	14.344333
22.855742	1210.692608	14.349351
22.314586	1198.785221	14.354368
22.262526	1203.919707	14.359386
22.501462	1196.800198	14.364403
22.480757	1203.416110	14.369421
22.900935	1204.596411	14.374439
22.818738	1205.178897	14.379456
22.881663	1208.778732	14.384474
22.973969	1209.501691	14.389491
22.918776	1204.686259	14.394509
22.755612	1188.330092	14.399527
22.879319	1195.363392	14.404544
22.766278	1198.590189	14.409562
22.839026	1187.306880	14.414579
22.927711	1194.740572	14.419597
22.946346	1188.288524	14.424615
22.752587	1180.322583	14.429632
22.978784	1191.279743	14.434650
22.626992	1193.736127	14.439667
22.914749	1193.477859	14.444685
23.007673	1190.814182	14.449703
23.133696	1202.911979	14.454720
22.994504	1196.772947	14.459738
23.329967	1203.840115	14.464755
23.235766	1198.115454	14.469773
23.122161	1182.602351	14.474791
22.835478	1177.035805	14.479808
22.828967	1186.639600	14.484826
22.880339	1193.047395	14.489843
23.062226	1203.781983	14.494861
23.303004	1199.996812	14.499879
22.852899	1204.444489	14.504896
22.910815	1199.713260	14.509914
23.126602	1206.848277	14.514931
22.992591	1207.555424	14.519949
23.216740	1195.898769	14.524967
23.187195	1203.661191	14.529984
23.093951	1205.060222	14.535002
23.322620	1190.228657	14.540019
22.938199	1202.930080	14.545037
23.077532	1174.041267	14.550055
23.185007	1219.140713	14.555072
23.603940	1214.863106	14.560090
23.510008	1197.707844	14.565107
23.177672	1228.244416	14.570125
23.313534	1197.267243	14.575143
23.369806	1247.688333	14.580160
23.278936	1229.569903	14.585178
23.945036	1237.809677	14.590195
23.396157	1226.573572	14.595213
23.574213	1234.541989	14.600231
23.556990	1223.634777	14.605248
23.667758	1233.127095	14.610266
23.897717	1207.769175	14.615283
23.223651	1219.650117	14.620301
23.910972	1211.658461	14.625319
23.880290	1218.692801	14.630336
23.868124	1213.595238	14.635354
23.480573	1206.542610	14.640371
23.456988	1204.048515	14.645389
24.067615	1203.260579	14.650407
23.591975	1204.753629	14.655424
23.646089	1213.130317	14.660442
23.881333	1226.305481	14.665459
23.958887	1215.089020	14.670477
23.728990	1231.256180	14.675495
23.868827	1218.749407	14.680512
23.762280	1212.136425	14.685530
24.226476	1228.685212	14.690547
23.839772	1220.347348	14.695565
23.964175	1218.979469	14.700583
23.744426	1213.647613	14.705600
24.051509	1225.751157	14.710618
24.099780	1223.385590	14.715635
24.101888	1227.278259	14.720653
24.104545	1211.968366	14.725671
24.103344	1233.123027	14.730688
24.138492	1220.022648	14.735706
23.981991	1208.264679	14.740723
23.759479	1220.591101	14.745741
23.977201	1229.695144	14.750759
24.174997	1237.149207	14.755776
24.147674	1220.724151	14.760794
24.172670	1227.905337	14.765811
24.173903	1230.675065	14.770829
24.477945	1217.994247	14.775847
24.367732	1237.753800	14.780864
24.130241	1225.009915	14.785882
24.199277	1226.700801	14.790899
23.900305	1234.850684	14.795917
24.469646	1215.788597	14.800935
24.617214	1223.412676	14.805952
24.172977	1237.333261	14.810970
24.320722	1221.419802	14.815987
24.190587	1228.499895	14.821005
24.292952	1228.680159	14.826023
24.402389	1235.292632	14.831040
24.619114	1218.965501	14.836058
24.889682	1232.509398	14.841075
24.131351	1234.887488	14.846093
24.676136	1219.964580	14.851111
24.239119	1229.069232	14.856128
24.020254	1227.296799	14.861146
24.296831	1223.161438	14.866163
24.576589	1255.848181	14.871181
24.726460	1247.736167	14.876199
24.804635	1266.197919	14.881216
25.060468	1248.179892	14.886234
24.923062	1241.781020	14.891251
24.648816	1238.184939	14.896269
24.486161	1239.423593	14.901287
24.804435	1235.799077	14.906304
24.338217	1238.934354	14.911322
24.782971	1266.572397	14.916339
24.699609	1252.998557	14.921357
24.715816	1282.068722	14.926375
24.486994	1242.717040	14.931392
24.848875	1267.324655	14.936410
25.064518	1253.863567	14.941427
24.789098	1253.271996	14.946445
25.096966	1261.740369	14.951463
25.145983	1252.121825	14.956480
25.016765	1254.136901	14.961498
25.280023	1266.510151	14.966515
25.221911	1261.216989	14.971533
25.267680	1251.620985	14.976551
24.921371	1267.805178	14.981568
25.318120	1257.956574	14.986586
25.350943	1241.031143	14.991603
25.227563	1262.368919	14.996621
25.084365	1264.744858	15.001639
25.372849	1254.820720	15.006656
25.322973	1262.767305	15.011674
25.251622	1250.589901	15.016691
25.137487	1246.897499	15.021709
25.258787	1262.480172	15.026727
25.212987	1248.330939	15.031744
25.190502	1247.845312	15.036762
25.700231	1259.100206	15.041779
25.307668	1238.812027	15.046797
25.369394	1262.600813	15.051815
25.441729	1250.719801	15.056832
25.454450	1252.004414	15.061850
25.581027	1251.018410	15.066867
25.177352	1248.792556	15.071885
25.310162	1264.082400	15.076903
25.136510	1256.262640	15.081920
25.294291	1248.415192	15.086938
25.584312	1238.610363	15.091955
25.088462	1252.345722	15.096973
24.981486	1261.076875	15.101991
25.675781	1241.307448	15.107008
25.405726	1298.719020	15.112026
25.808378	1266.456518	15.117043
25.572506	1284.323472	15.122061
25.798608	1283.186320	15.127079
25.632867	1276.851723	15.132096
25.830679	1254.891697	15.137114
25.713242	1294.169600	15.142131
25.816388	1277.245494	15.147149
25.647511	1274.437948	15.152167
26.007875	1287.877917	15.157184
26.033246	1273.670120	15.162202
25.964380	1282.222184	15.167219
26.069096	1272.719006	15.172237
25.889514	1283.679608	15.177255
26.359094	1273.712418	15.182272
25.931363	1266.290234	15.187290
26.123458	1279.936348	15.192307
26.437316	1258.514632	15.197325
26.013750	1275.398533	15.202343
26.551897	1247.274911	15.207360
25.810564	1237.356160	15.212378
26.134166	1237.910105	15.217395
25.934913	1237.035841	15.222413
26.244602	1266.019844	15.227431
26.291368	1256.137401	15.232448
26.168237	1253.827479	15.237466
26.376998	1238.549178	15.242483
26.113842	1262.237203	15.247501
25.971819	1244.460377	15.252519
26.400419	1275.762830	15.257536
26.357343	1262.383893	15.262554
26.422199	1282.656679	15.267571
26.521070	1272.212238	15.272589
26.639384	1269.050592	15.277607
26.491227	1242.195699	15.282624
26.289490	1238.960841	15.287642
26.393583	1241.424745	15.292659
26.350328	1256.486272	15.297677
26.381677	1274.862700	15.302695
26.400664	1278.900547	15.307712
26.643744	1276.536934	15.312730
26.732177	1274.558191	15.317747
26.438781	1277.927022	15.322765
26.451913	1292.060991	15.327783
26.575417	1274.911856	15.332800
25.994530	1280.313172	15.337818
26.178244	1285.837926	15.342835
26.246800	1273.559541	15.347853
26.551168	1257.943517	15.352871
26.805981	1257.397935	15.357888
26.509487	1319.348608	15.362906
26.763156	1303.389853	15.367923
27.230913	1275.368635	15.372941
27.070903	1303.214881	15.377959
27.003466	1292.452473	15.382976
26.696448	1266.244186	15.387994
26.930669	1290.776253	15.393011
27.039820	1246.384408	15.398029
26.706285	1305.670072	15.403047
26.891198	1282.434825	15.408064
26.848256	1319.067799	15.413082
27.151014	1309.566044	15.418099
27.059673	1295.831422	15.423117
26.892022	1311.984025	15.428135
27.312091	1303.553620	15.433152
26.868836	1302.499626	15.438170
27.372093	1303.974984	15.443187
27.606561	1293.840794	15.448205
27.039277	1288.422771	15.453223
27.333199	1307.007462	15.458240
27.383220	1294.643931	15.463258
27.334022	1273.393348	15.468275
27.235811	1293.336670	15.473293
26.987325	1275.197704	15.478311
27.308657	1279.196769	15.483328
27.129841	1302.468734	15.488346
27.171220	1310.547076	15.493363
27.465807	1298.729674	15.498381
27.321756	1292.597668	15.503399
27.438242	1294.656929	15.508416
27.268712	1292.834150	15.513434
27.301650	1302.680256	15.518451
27.847843	1304.015066	15.523469
27.370825	1312.473374	15.528487
27.620511	1293.979666	15.533504
26.822200	1305.468380	15.538522
27.244025	1300.501335	15.543539
27.381267	1284.584763	15.548557
27.217174	1322.290943	15.553575
27.756312	1323.291841	15.558592
28.029710	1323.984352	15.563610
28.216704	1340.467372	15.568627
28.304782	1308.409096	15.573645
28.056785	1307.898088	15.578663
28.080509	1301.084972	15.583680
27.918645	1292.546047	15.588698
28.059785	1282.972562	15.593715
28.328404	1289.682363	15.598733
28.037781	1286.394034	15.603751
27.780556	1282.718152	15.608768
27.852948	1291.574866	15.613786
27.967202	1287.218423	15.618803
27.901218	1279.153400	15.623821
27.726603	1289.933899	15.628839
28.298049	1289.753076	15.633856
28.203295	1288.536541	15.638874
28.010542	1286.380856	15.643891
28.107880	1286.834043	15.648909
27.854063	1297.591001	15.653927
28.118767	1290.637216	15.658944
28.163459	1296.146395	15.663962
28.031395	1288.996353	15.668979
28.149171	1296.450625	15.673997
28.218615	1291.401364	15.679015
28.192881	1284.814784	15.684032
28.317521	1292.892421	15.689050
28.233284	1296.561363	15.694067
28.316648	1290.017153	15.699085
28.221157	1300.939190	15.704103
28.316062	1307.528847	15.709120
28.605472	1304.785052	15.714138
28.380161	1317.665682	15.719155
28.753095	1324.319539	15.724173
28.440980	1305.827330	15.729191
28.737061	1284.402119	15.734208
28.315508	1304.349837	15.739226
28.455362	1305.298015	15.744243
28.686143	1304.427517	15.749261
28.646017	1313.522402	15.754279
28.936975	1312.107503	15.759296
28.664064	1333.422043	15.764314
28.393040	1307.785215	15.769331
28.932503	1297.278352	15.774349
28.941249	1329.082017	15.779367
29.132400	1320.895741	15.784384
28.956076	1306.094044	15.789402
28.639422	1295.703273	15.794419
28.715531	1287.905006	15.799437
28.838597	1295.918405	15.804455
28.876209	1310.929341	15.809472
28.978250	1315.281126	15.814490
28.805424	1314.777004	15.819507
28.794708	1320.952524	15.824525
28.808934	1330.980951	15.829543
29.118345	1324.878851	15.834560
29.212582	1311.660432	15.839578
29.385541	1320.015082	15.844595
29.523029	1312.301390	15.849613
29.333497	1310.162490	15.854631
29.059452	1292.776303	15.859648
29.484211	1283.373079	15.864666
29.185233	1298.863953	15.869683
29.308138	1270.378669	15.874701
29.081205	1283.265819	15.879719
29.149664	1269.911556	15.884736
29.370903	1288.399282	15.889754
29.053573	1309.651662	15.894771
29.560132	1304.911764	15.899789
29.252636	1322.283697	15.904807
29.214626	1324.499731	15.909824
29.491091	1321.775299	15.914842
29.250146	1313.025614	15.919859
29.531227	1314.330351	15.924877
29.410482	1324.322100	15.929895
29.483838	1303.548980	15.934912
29.304495	1320.265000	15.939930
29.353267	1320.818738	15.944947
29.346354	1312.659337	15.949965
29.156061	1323.922112	15.954983
29.515228	1315.919819	15.960000
29.412528	1316.942860	15.965018
29.570389	1332.250803	15.970035
29.775773	1350.267677	15.975053
29.723164	1325.610539	15.980071
29.773707	1358.997860	15.985088
30.180462	1336.460143	15.990106
29.665926	1341.737646	15.995123
30.068439	1346.447343	16.000141
29.941937	1341.890191	16.005159
30.111205	1330.119490	16.010176
30.072260	1345.998359	16.015194
30.005567	1339.006172	16.020211
30.267360	1334.019023	16.025229
29.783576	1324.545178	16.030247
30.273147	1318.603103	16.035264
30.167153	1329.515826	16.040282
29.992952	1310.270192	16.045299
29.765803	1354.102148	16.050317
29.885290	1327.122618	16.055335
30.106052	1336.536116	16.060352
30.091672	1337.241493	16.065370
30.044604	1332.358657	16.070387
30.197135	1338.597807	16.075405
30.230546	1322.007227	16.080423
30.088083	1336.735464	16.085440
30.251505	1339.944941	16.090458
29.959021	1345.592853	16.095475
30.473264	1335.340085	16.100493
30.580026	1338.663986	16.105511
30.539138	1332.990541	16.110528
30.636734	1334.280501	16.115546
30.408813	1346.213081	16.120563
30.530817	1325.218249	16.125581
30.233883	1342.506729	16.130599
30.157284	1357.872540	16.135616
30.528847	1355.589093	16.140634
30.515791	1382.457269	16.145651
30.491628	1372.265176	16.150669
30.566646	1377.143513	16.155687
30.897546	1372.783951	16.160704
30.975156	1360.263386	16.165722
30.760627	1380.072802	16.170739
30.940262	1370.966581	16.175757
31.094831	1366.770417	16.180775
31.176643	1374.829763	16.185792
31.360200	1358.556527	16.190810
30.994585	1348.853043	16.195827
31.013197	1347.336863	16.200845
30.969058	1325.767659	16.205863
30.941794	1337.419704	16.210880
31.318552	1317.469592	16.215898
31.034339	1341.203575	16.220915
30.819678	1340.391533	16.225933
30.772799	1359.716453	16.230951
30.713254	1357.816353	16.235968
31.030152	1366.097739	16.240986
31.042333	1381.674349	16.246003
31.100029	1371.156183	16.251021
31.151012	1352.437699	16.256039
31.110756	1381.326741	16.261056
30.929683	1352.894495	16.266074
30.901877	1381.290789	16.271091
31.170609	1371.917111	16.276109
31.251213	1375.680902	16.281127
31.121819	1393.877060	16.286144
31.338780	1393.131452	16.291162
31.463000	1394.500537	16.296179
31.379367	1394.801700	16.301197
31.452129	1399.425584	16.306215
31.360250	1399.973444	16.311232
31.568475	1401.440812	16.316250
31.503223	1410.635716	16.321267
31.590995	1387.618706	16.326285
31.515619	1398.680748	16.331303
31.699777	1388.847086	16.336320
31.980489	1399.292364	16.341338
31.871645	1396.149617	16.346355
31.765150	1382.098018	16.351373
31.603819	1410.712285	16.356391
31.935986	1390.962659	16.361408
31.852914	1386.739899	16.366426
31.743657	1409.942743	16.371443
31.861681	1392.530085	16.376461
31.621002	1410.316166	16.381479
31.810457	1388.781970	16.386496
32.070120	1391.927348	16.391514
31.762512	1410.686756	16.396531
31.757167	1403.826320	16.401549
32.172584	1429.413495	16.406567
32.122207	1440.565960	16.411584
32.398344	1426.100950	16.416602
32.265329	1426.509086	16.421619
32.286052	1425.469170	16.426637
32.291903	1415.118109	16.431655
32.069170	1409.385550	16.436672
32.290487	1420.414447	16.441690
32.318593	1424.111121	16.446707
32.331075	1420.859360	16.451725
32.249848	1421.188452	16.456743
32.491610	1429.412648	16.461760
32.744263	1410.111388	16.466778
32.277173	1429.220285	16.471795
32.726490	1419.369482	16.476813
32.689474	1406.602900	16.481831
32.157357	1420.130277	16.486848
32.505438	1427.713048	16.491866
32.556018	1402.257560	16.496883
32.383159	1420.166539	16.501901
32.806029	1406.294749	16.506919
32.800356	1425.652509	16.511936
33.009256	1423.651388	16.516954
32.899739	1404.378010	16.521971
33.025702	1416.582958	16.526989
33.046463	1404.461516	16.532007
32.627235	1396.369398	16.537024
32.601555	1386.024960	16.542042
32.927195	1427.610877	16.547059
32.749517	1406.278346	16.552077
32.423058	1432.775045	16.557095
33.027402	1413.401963	16.562112
32.760312	1416.083964	16.567130
33.131638	1404.372210	16.572147
33.115626	1438.169860	16.577165
33.201258	1398.799060	16.582183
33.034214	1402.997167	16.587200
33.087389	1416.478384	16.592218
33.523636	1422.760408	16.597235
33.349368	1410.957918	16.602253
33.371173	1399.704589	16.607271
33.069294	1425.701872	16.612288
33.400992	1411.567776	16.617306
33.293863	1394.799760	16.622323
33.210190	1428.230667	16.627341
33.339088	1398.018635	16.632359
33.215689	1431.624193	16.637376
33.478923	1385.269456	16.642394
33.585718	1390.996846	16.647411
33.371736	1439.366525	16.652429
33.445889	1399.016024	16.657447
33.448619	1426.463761	16.662464
33.380090	1396.530174	16.667482
33.092072	1423.571262	16.672499
33.294975	1402.487914	16.677517
33.833604	1433.694516	16.682535
33.497817	1425.327962	16.687552
33.456967	1441.642950	16.692570
33.812688	1443.778905	16.697587
33.723097	1428.607759	16.702605
33.927890	1468.352250	16.707623
33.587923	1433.249060	16.712640
33.898207	1447.887901	16.717658
33.858537	1433.018663	16.722675
33.547431	1416.652799	16.727693
33.969475	1451.805723	16.732711
33.525279	1431.321020	16.737728
33.918551	1428.005381	16.742746
33.461001	1457.149882	16.747763
34.231316	1438.624867	16.752781
34.086247	1471.991737	16.757799
34.128506	1441.996344	16.762816
34.463877	1463.945494	16.767834
34.327700	1450.769986	16.772851
33.867335	1471.929015	16.777869
34.474039	1434.291796	16.782887
34.449366	1479.987264	16.787904
34.237737	1451.300157	16.792922
34.376197	1450.696050	16.797939
34.492389	1443.411959	16.802957
34.477278	1472.169762	16.807975
34.267492	1455.389735	16.812992
34.656383	1456.265174	16.818010
34.423266	1440.538054	16.823027
34.546818	1463.746325	16.828045
34.852095	1434.533236	16.833063
34.852911	1468.554780	16.838080
35.111185	1455.442198	16.843098
34.983054	1441.096701	16.848115
34.926832	1454.980778	16.853133
34.793146	1423.331982	16.858151
34.688168	1429.023951	16.863168
35.099019	1424.799482	16.868186
34.813072	1410.727713	16.873203
34.364406	1412.935324	16.878221
34.894676	1445.790177	16.883239
35.120904	1442.037151	16.888256
34.916747	1447.346985	16.893274
35.318340	1449.801229	16.898291
34.754661	1425.396882	16.903309
34.986911	1445.588147	16.908327
34.863988	1450.299883	16.913344
34.916000	1441.047237	16.918362
35.135531	1440.092013	16.923379
34.998053	1455.832566	16.928397
35.377615	1436.550355	16.933415
35.165040	1446.039328	16.938432
35.064877	1451.785592	16.943450
35.276811	1445.194067	16.948467
34.887866	1438.975217	16.953485
35.142595	1447.156457	16.958503
35.115874	1457.984278	16.963520
35.223440	1451.522648	16.968538
35.479257	1469.080187	16.973555
35.403884	1475.234625	16.978573
35.557429	1473.822750	16.983591
35.997781	1476.347894	16.988608
35.548268	1477.382213	16.993626
35.869963	1464.940604	16.998643
35.745878	1440.788580	17.003661
36.024331	1431.399157	17.008679
35.678982	1465.683534	17.013696
35.454322	1431.016547	17.018714
35.837113	1442.364188	17.023731
35.378678	1442.220204	17.028749
35.524502	1472.103752	17.033767
35.647560	1471.566592	17.038784
35.590028	1482.534620	17.043802
35.687735	1477.537413	17.048819
35.723839	1489.939219	17.053837
36.065099	1462.552846	17.058855
35.626971	1497.780146	17.063872
35.814753	1468.991553	17.068890
36.292868	1490.240028	17.073907
36.173523	1485.853142	17.078925
36.035385	1490.343956	17.083943
36.249809	1478.756263	17.088960
35.984709	1502.910590	17.093978
36.828588	1494.207999	17.098995
36.228896	1481.487046	17.104013
36.319439	1483.671591	17.109031
36.615387	1464.923331	17.114048
36.387560	1493.845659	17.119066
36.456235	1453.222183	17.124083
36.209702	1489.664698	17.129101
36.555824	1501.457092	17.134119
36.769742	1462.466768	17.139136
36.496780	1494.856826	17.144154
36.773727	1466.928588	17.149171
36.611252	1469.096856	17.154189
36.709576	1465.617471	17.159207
36.488607	1480.471627	17.164224
36.501043	1466.267277	17.169242
37.066399	1470.472862	17.174259
36.832232	1512.673676	17.179277
36.816108	1476.825050	17.184295
36.920896	1502.746604	17.189312
36.915172	1490.335169	17.194330
37.161132	1515.482351	17.199347
37.058503	1471.070112	17.204365
36.688311	1492.771621	17.209383
36.785931	1496.482395	17.214400
36.600832	1502.308289	17.219418
37.205019	1499.124160	17.224435
37.229985	1497.779979	17.229453
37.141772	1502.566417	17.234471
37.143886	1492.977216	17.239488
36.922469	1496.262260	17.244506
37.221252	1495.267652	17.249523
37.254699	1499.447969	17.254541
37.272634	1487.935648	17.259559
37.323322	1505.187757	17.264576
37.167791	1500.507773	17.269594
37.330043	1476.108685	17.274611
36.952957	1508.255838	17.279629
37.033026	1520.185058	17.284647
37.292934	1505.827947	17.289664
37.417183	1531.659935	17.294682
37.632805	1528.059584	17.299699
37.443363	1530.664730	17.304717
37.639378	1531.050280	17.309735
37.478232	1525.079771	17.314752
37.513976	1529.453206	17.319770
38.104584	1503.979051	17.324787
37.728058	1534.049849	17.329805
38.114872	1528.289241	17.334823
38.007806	1502.846133	17.339840
37.647120	1538.312856	17.344858
37.856928	1527.598862	17.349875
37.825464	1521.116904	17.354893
38.025051	1539.363021	17.359911
37.618730	1527.613173	17.364928
37.572987	1541.541278	17.369946
37.917160	1530.569907	17.374963
38.022135	1575.807714	17.379981
37.952795	1536.072730	17.384999
38.380944	1570.572184	17.390016
38.495926	1543.080179	17.395034
38.893143	1565.655104	17.400051
38.477000	1525.912537	17.405069
38.239499	1525.391981	17.410087
38.360891	1522.483039	17.415104
38.196834	1533.169228	17.420122
38.715263	1532.546990	17.425139
38.763159	1541.780559	17.430157
38.384264	1532.568264	17.435175
38.509415	1523.962978	17.440192
38.515446	1524.363097	17.445210
38.867808	1547.533439	17.450227
38.423696	1556.291796	17.455245
38.491676	1549.793966	17.460263
38.860637	1526.991431	17.465280
38.497236	1564.119711	17.470298
38.844620	1527.464249	17.475315
38.396428	1557.104518	17.480333
38.721992	1536.361626	17.485351
38.852898	1542.310167	17.490368
38.805525	1551.357595	17.495386
39.237846	1531.771125	17.500403
39.023321	1558.904561	17.505421
38.845055	1556.822026	17.510439
38.932031	1541.141271	17.515456
38.476568	1565.873458	17.520474
39.170418	1551.785287	17.525491
39.458133	1560.220873	17.530509
38.946491	1576.979959	17.535527
39.305568	1561.805544	17.540544
39.064148	1568.445813	17.545562
39.282237	1590.509025	17.550579
39.658364	1581.349314	17.555597
39.623632	1573.693623	17.560615
39.644107	1577.930299	17.565632
39.458904	1581.458118	17.570650
39.754936	1569.943065	17.575667
39.479756	1545.667103	17.580685
39.169101	1555.543011	17.585703
39.941412	1562.216654	17.590720
39.645409	1563.364919	17.595738
39.692434	1583.718834	17.600755
39.962451	1550.378128	17.605773
39.834985	1570.538849	17.610791
39.726796	1545.569312	17.615808
39.724354	1546.559076	17.620826
39.960554	1548.531644	17.625843
40.330566	1560.889696	17.630861
39.940206	1528.619380	17.635879
40.235735	1519.093475	17.640896
39.909360	1529.511402	17.645914
39.990246	1521.834941	17.650931
40.225300	1529.218723	17.655949
39.990426	1513.689997	17.660967
39.937075	1533.019327	17.665984
40.089117	1524.093584	17.671002
39.984535	1559.802652	17.676019
40.406146	1524.601375	17.681037
40.063186	1572.397483	17.686055
40.233757	1551.322222	17.691072
40.036898	1554.136187	17.696090
40.232236	1561.677326	17.701107
40.034875	1573.827008	17.706125
40.217218	1556.962303	17.711143
40.136153	1554.588995	17.716160
40.350359	1571.514666	17.721178
40.568777	1566.134820	17.726195
40.962089	1588.512995	17.731213
40.589166	1587.389559	17.736231
40.800412	1590.427875	17.741248
40.835386	1592.295692	17.746266
40.695444	1582.362581	17.751283
40.968608	1576.103356	17.756301
41.024386	1578.297392	17.761319
40.740311	1560.144080	17.766336
40.716715	1576.034910	17.771354
40.888420	1582.639972	17.776371
41.030032	1589.519603	17.781389
40.994381	1583.255357	17.786407
41.102281	1593.442054	17.791424
41.013296	1589.594547	17.796442
40.809717	1591.564900	17.801459
41.201464	1583.242670	17.806477
41.155907	1590.762468	17.811495
41.325382	1582.373442	17.816512
41.104216	1579.143178	17.821530
40.984439	1585.202500	17.826547
41.396011	1583.590594	17.831565
41.215166	1590.310872	17.836583
41.355402	1587.027688	17.841600
41.412059	1575.640466	17.846618
41.306456	1604.319372	17.851635
41.722801	1619.974924	17.856653
41.580216	1611.596324	17.861671
41.868065	1601.462845	17.866688
41.870535	1614.607851	17.871706
41.290049	1598.473499	17.876723
41.920453	1593.572191	17.881741
41.579065	1604.683106	17.886759
41.721010	1614.733831	17.891776
42.015373	1599.631830	17.896794
42.041287	1601.752770	17.901811
42.332479	1603.703992	17.906829
42.110935	1605.943046	17.911847
42.211960	1578.778806	17.916864
42.031273	1568.108970	17.921882
41.766157	1588.596041	17.926899
42.162922	1586.149669	17.931917
42.194938	1596.173870	17.936935
41.958337	1595.503734	17.941952
42.392007	1603.286875	17.946970
42.025869	1604.125439	17.951987
42.244333	1615.829752	17.957005
42.308675	1603.822313	17.962023
42.460351	1597.905701	17.967040
42.512350	1604.601435	17.972058
42.522184	1607.813445	17.977075
42.529028	1602.081947	17.982093
42.753478	1598.593426	17.987111
42.561709	1607.162136	17.992128
42.679726	1608.148424	17.997146
42.663798	1603.847253	18.002163
42.690784	1600.670214	18.007181
42.706351	1608.669472	18.012199
42.692540	1599.936869	18.017216
42.774643	1606.341520	18.022234
42.720661	1610.700975	18.027251
42.577422	1600.861184	18.032269
42.526085	1608.564379	18.037287
42.825143	1609.624039	18.042304
42.876245	1615.228270	18.047322
42.642436	1625.024331	18.052339
42.953308	1631.458574	18.057357
42.907054	1649.832125	18.062375
43.087316	1614.077679	18.067392
42.795938	1647.405367	18.072410
43.421240	1637.995102	18.077427
43.331323	1629.431918	18.082445
43.400743	1640.356224	18.087463
43.489810	1634.984398	18.092480
43.123477	1621.416014	18.097498
43.508248	1645.721761	18.102515
43.474772	1612.887837	18.107533
43.099830	1662.584789	18.112551
43.534183	1635.040103	18.117568
43.425663	1652.213960	18.122586
43.612492	1656.731648	18.127603
43.951400	1647.637606	18.132621
43.961114	1653.482828	18.137639
43.860570	1648.770431	18.142656
43.765515	1643.092919	18.147674
43.803473	1644.115572	18.152691
44.378255	1637.763388	18.157709
44.146785	1646.461145	18.162727
44.013592	1626.297790	18.167744
43.943483	1617.119562	18.172762
43.793208	1638.762622	18.177779
44.102685	1636.289266	18.182797
44.030798	1637.154835	18.187815
44.171390	1657.834484	18.192832
44.325983	1634.026222	18.197850
44.039409	1634.347170	18.202867
44.166504	1653.427665	18.207885
44.641647	1643.706297	18.212903
44.503661	1645.502606	18.217920
44.880322	1639.232353	18.222938
44.597723	1635.978840	18.227955
44.430754	1633.916514	18.232973
44.454880	1628.948294	18.237991
44.628800	1634.654065	18.243008
44.591199	1635.017103	18.248026
44.645956	1637.536133	18.253043
44.866345	1651.229996	18.258061
45.043775	1649.167798	18.263079
44.428402	1631.975631	18.268096
44.643324	1645.377786	18.273114
44.798443	1645.272797	18.278131
45.028003	1646.296354	18.283149
45.078629	1630.574109	18.288167
44.837445	1644.190571	18.293184
45.088493	1643.279071	18.298202
44.791064	1634.321125	18.303219
45.338974	1646.641443	18.308237
45.134009	1648.251810	18.313255
44.896604	1630.417361	18.318272
45.101185	1634.990412	18.323290
44.944548	1644.222060	18.328307
45.113552	1631.653653	18.333325
44.818375	1632.757747	18.338343
44.879318	1671.224878	18.343360
45.486557	1658.575547	18.348378
44.815564	1687.679046	18.353395
45.322873	1662.298122	18.358413
45.152290	1665.710373	18.363431
45.496047	1690.924061	18.368448
45.757476	1687.759950	18.373466
45.811853	1695.754639	18.378483
45.783744	1700.109995	18.383501
46.112818	1691.225129	18.388519
45.851359	1676.760664	18.393536
45.907588	1679.498113	18.398554
45.630488	1677.708168	18.403571
45.929921	1670.861920	18.408589
45.951642	1698.936341	18.413607
45.775403	1679.069208	18.418624
45.953464	1699.327671	18.423642
46.200842	1680.706427	18.428659
46.554380	1680.079022	18.433677
46.726497	1689.747470	18.438695
46.587871	1692.509704	18.443712
46.614415	1676.528561	18.448730
46.455657	1663.247924	18.453747
46.340699	1658.323896	18.458765
46.634270	1656.685184	18.463783
46.435233	1659.109416	18.468800
46.562296	1631.695538	18.473818
46.317178	1654.942464	18.478835
46.358756	1655.380961	18.483853
46.593321	1665.975363	18.488871
46.422163	1677.605012	18.493888
46.924731	1682.690541	18.498906
46.422304	1696.468262	18.503923
46.636676	1683.760443	18.508941
46.775816	1690.720739	18.513959
46.387772	1696.557055	18.518976
46.883776	1684.639581	18.523994
46.773041	1681.890320	18.529011
46.488913	1687.071424	18.534029
46.289645	1699.646224	18.539047
46.587298	1712.646717	18.544064
46.877577	1711.098186	18.549082
46.953972	1718.806237	18.554099
47.154887	1715.464585	18.559117
47.352983	1722.519313	18.564135
47.408582	1717.638849	18.569152
47.648355	1711.769488	18.574170
47.332225	1718.887346	18.579187
47.459621	1715.469331	18.584205
47.469612	1714.769300	18.589223
47.202352	1728.688868	18.594240
47.564923	1727.853958	18.599258
47.613888	1742.824206	18.604275
48.111744	1736.680873	18.609293
48.072388	1729.902784	18.614311
47.830702	1730.795437	18.619328
48.118935	1710.302065	18.624346
47.864209	1710.128734	18.629363
47.952661	1715.494244	18.634381
47.780553	1717.536672	18.639399
47.636354	1710.367905	18.644416
47.968012	1714.724092	18.649434
48.132427	1733.614700	18.654451
47.823931	1743.863191	18.659469
48.350840	1736.574801	18.664487
47.956485	1744.617485	18.669504
48.320757	1728.959944	18.674522
48.278499	1735.153254	18.679539
48.243290	1733.115518	18.684557
48.205377	1743.748712	18.689575
48.273224	1742.359917	18.694592
48.481628	1730.124909	18.699610
48.492126	1742.131474	18.704627
48.341416	1741.151908	18.709645
48.362216	1726.524404	18.714663
48.381939	1744.152964	18.719680
48.669018	1735.208702	18.724698
48.653418	1742.659309	18.729715
48.910594	1758.198827	18.734733
48.853354	1757.691984	18.739751
48.408026	1776.816740	18.744768
48.982616	1765.887097	18.749786
48.964157	1780.119388	18.754803
49.047569	1778.421372	18.759821
49.300087	1775.296416	18.764839
48.985908	1775.777496	18.769856
49.214485	1767.278266	18.774874
48.806188	1770.715868	18.779891
48.892983	1773.692275	18.784909
49.314311	1764.687261	18.789927
49.093818	1766.540786	18.794944
48.999281	1753.946663	18.799962
49.131610	1757.755787	18.804979
49.273028	1763.718474	18.809997
49.707761	1767.477801	18.815015
49.375121	1775.104825	18.820032
49.690174	1789.927296	18.825050
49.842129	1772.576410	18.830067
49.907177	1776.654241	18.835085
49.823586	1780.548141	18.840103
49.547036	1773.013492	18.845120
50.191274	1765.585256	18.850138
49.991012	1761.283548	18.855155
50.123680	1763.354454	18.860173
50.076277	1754.068700	18.865191
50.051553	1749.617881	18.870208
49.694232	1749.314621	18.875226
49.992269	1754.396615	18.880243
49.831953	1763.068937	18.885261
50.244840	1765.631548	18.890279
50.291297	1780.729649	18.895296
50.354080	1771.089689	18.900314
50.476741	1782.200665	18.905331
50.546524	1774.204948	18.910349
50.194779	1777.701171	18.915367
50.243437	1774.762881	18.920384
50.133081	1766.536351	18.925402
50.391750	1767.569431	18.930419
50.378874	1772.117432	18.935437
50.519587	1774.249976	18.940455
50.664629	1800.448785	18.945472
50.782690	1796.478542	18.950490
50.671283	1797.194696	18.955507
50.832239	1807.855996	18.960525
51.112211	1801.113463	18.965543
50.833599	1800.372938	18.970560
50.989325	1804.258566	18.975578
51.263908	1790.982635	18.980595
51.065719	1806.810327	18.985613
51.311207	1795.967752	18.990631
50.650323	1807.260331	18.995648
51.305662	1796.497111	19.000666
51.301525	1790.252916	19.005683
50.923980	1797.312967	19.010701
51.408734	1797.565963	19.015719
50.915466	1797.440110	19.020736
51.173558	1794.449540	19.025754
51.270598	1799.055524	19.030771
51.410913	1814.042738	19.035789
51.591866	1820.132849	19.040807
51.811960	1835.516344	19.045824
52.047298	1814.329699	19.050842
51.832459	1817.409274	19.055859
51.779825	1825.847386	19.060877
51.799548	1831.227046	19.065895
51.913556	1824.825571	19.070912
51.731229	1823.969017	19.075930
51.824339	1832.080300	19.080947
51.694290	1832.863921	19.085965
52.017625	1825.348406	19.090983
51.708065	1833.520760	19.096000
52.050169	1824.515759	19.101018
51.965674	1819.976924	19.106035
51.548525	1839.265580	19.111053
52.257689	1857.204320	19.116071
52.029043	1846.904505	19.121088
51.881599	1869.143627	19.126106
51.909973	1860.191783	19.131123
52.373824	1867.621048	19.136141
52.769121	1879.698493	19.141159
52.560599	1881.779783	19.146176
53.107602	1893.076426	19.151194
53.239842	1861.502238	19.156211
52.914130	1878.217074	19.161229
53.050678	1840.115815	19.166247
53.053831	1866.925677	19.171264
52.851577	1833.784690	19.176282
52.891984	1869.076572	19.181299
52.912531	1829.107799	19.186317
52.993496	1859.296644	19.191335
53.082511	1852.789032	19.196352
53.202271	1868.298674	19.201370
53.770560	1857.148174	19.206387
53.204272	1868.419422	19.211405
53.477131	1849.186716	19.216423
53.451642	1843.444549	19.221440
53.287112	1856.045404	19.226458
53.369014	1859.090248	19.231475
53.459382	1860.332645	19.236493
53.762462	1859.011718	19.241511
53.849321	1881.496635	19.246528
53.563004	1876.496041	19.251546
54.041579	1867.752393	19.256563
53.939184	1871.957627	19.261581
53.996274	1866.046553	19.266599
53.769424	1854.244219	19.271616
53.680912	1858.241171	19.276634
53.881427	1850.620962	19.281651
53.707488	1860.327409	19.286669
53.833565	1861.365912	19.291687
53.869791	1858.892053	19.296704
54.279504	1865.058958	19.301722
54.337911	1847.353243	19.306739
53.917423	1863.114202	19.311757
53.918182	1866.602994	19.316775
53.998261	1852.810616	19.321792
54.087537	1880.209232	19.326810
54.510436	1888.448850	19.331827
54.791979	1894.036888	19.336845
54.776245	1880.865375	19.341863
54.752348	1905.785715	19.346880
54.845075	1870.381223	19.351898
54.775727	1893.116010	19.356915
54.395648	1879.497665	19.361933
54.886048	1884.692173	19.366951
54.720380	1889.214240	19.371968
54.452345	1887.134961	19.376986
54.805997	1891.270618	19.382003
54.832601	1883.775654	19.387021
55.055505	1876.535677	19.392039
55.255132	1882.514298	19.397056
54.711296	1902.633343	19.402074
54.962895	1893.567229	19.407091
55.002499	1915.377047	19.412109
54.966146	1910.169838	19.417127
55.174309	1931.389659	19.422144
55.064855	1935.265703	19.427162
55.021943	1926.520241	19.432179
54.914557	1950.538475	19.437197
55.563984	1930.389886	19.442215
55.463097	1973.959761	19.447232
55.237938	1959.591470	19.452250
55.830068	1956.431193	19.457267
56.094676	1955.833691	19.462285
55.720761	1961.046513	19.467303
56.098043	1946.534970	19.472320
56.256616	1948.567166	19.477338
56.164777	1941.676224	19.482355
56.109162	1952.178687	19.487373
56.380145	1955.397891	19.492391
56.549831	1944.268420	19.497408
56.396778	1929.673156	19.502426
56.528379	1928.472377	19.507443
56.259045	1949.181637	19.512461
56.208125	1948.894002	19.517479
56.481355	1931.559765	19.522496
56.534036	1933.555363	19.527514
56.500000	1923.611419	19.532531
56.379755	1932.809132	19.537549
56.666590	1938.962632	19.542567
56.674891	1934.698397	19.547584
56.381382	1951.611101	19.552602
56.814073	1929.099793	19.557619
56.577823	1924.182433	19.562637
56.680048	1963.815656	19.567655
57.090072	1948.699568	19.572672
56.851588	1966.765977	19.577690
56.783278	1967.102459	19.582707
57.103628	1986.177742	19.587725
57.301481	1959.322965	19.592743
57.217848	1987.774969	19.597760
57.177625	1959.029630	19.602778
57.222089	1975.926217	19.607795
57.284524	1988.870090	19.612813
56.969797	1963.201312	19.617831
57.517661	1978.122130	19.622848
57.505165	1967.392929	19.627866
57.594491	1953.067300	19.632883
57.244724	1969.463607	19.637901
57.571146	1985.465807	19.642919
57.739735	1983.351490	19.647936
57.606548	1991.330637	19.652954
57.912932	2011.970196	19.657971
57.651545	1987.557583	19.662989
57.625212	2007.594244	19.668007
58.013175	1985.481666	19.673024
57.890669	1982.178947	19.678042
57.949346	1994.690843	19.683059
57.989520	1989.911849	19.688077
58.100618	2005.078526	19.693095
58.829182	2010.829704	19.698112
58.517638	2012.183400	19.703130
58.775321	1997.585486	19.708147
58.591831	2009.502085	19.713165
58.361978	1966.709955	19.718183
58.482465	1995.827846	19.723200
58.753507	2003.865231	19.728218
58.954980	2005.830818	19.733235
58.729270	2014.339112	19.738253
58.847010	2023.116684	19.743271
58.914746	1987.602633	19.748288
58.453483	2029.595773	19.753306
58.901256	1995.268510	19.758323
59.312680	2000.093410	19.763341
59.130536	2025.894919	19.768359
59.481019	1999.324040	19.773376
59.316453	2015.643674	19.778394
59.769945	2005.733611	19.783411
59.563860	1993.079991	19.788429
59.257514	2022.081958	19.793447
59.590161	1985.783196	19.798464
59.263617	2022.112390	19.803482
59.728320	2009.916500	19.808499
59.224795	1992.205840	19.813517
59.348507	2012.762847	19.818535
59.496025	1989.898947	19.823552
59.537265	2026.383432	19.828570
59.677158	1984.446215	19.833587
59.366219	2024.082571	19.838605
59.761521	2003.109243	19.843623
59.681930	1994.808463	19.848640
59.493711	2043.289305	19.853658
59.777574	2017.204074	19.858675
60.260662	2033.506960	19.863693
60.297787	2032.124611	19.868711
59.851871	2032.480413	19.873728
59.859612	2038.865655	19.878746
60.198004	2030.617748	19.883763
60.133423	2038.776316	19.888781
60.209112	2054.916107	19.893799
60.568041	2069.456588	19.898816
60.353744	2052.091416	19.903834
60.611179	2056.250331	19.908851
60.828611	2068.342142	19.913869
60.536772	2054.533379	19.918887
60.611401	2067.380996	19.923904
60.684831	2035.491763	19.928922
60.661506	2079.147113	19.933939
60.964763	2055.531532	19.938957
60.994525	2068.979339	19.943975
61.139570	2092.743620	19.948992
61.073884	2065.823707	19.954010
61.073294	2095.857735	19.959027
61.666087	2080.709219	19.964045
61.643776	2075.049823	19.969063
61.551882	2086.612102	19.974080
61.456473	2083.899646	19.979098
61.671809	2064.867740	19.984115
61.497132	2091.602556	19.989133
61.338219	2068.726052	19.994151
61.074396	2085.970806	19.999168
61.302982	2087.290282	20.004186
61.583783	2098.926845	20.009203
61.829924	2079.773602	20.014221
61.622187	2103.919778	20.019239
62.081633	2115.628539	20.024256
62.079817	2108.317318	20.029274
62.401492	2124.182002	20.034291
62.465761	2115.974616	20.039309
61.911066	2121.873854	20.044327
62.180113	2135.396822	20.049344
62.250160	2097.607516	20.054362
62.053896	2128.871472	20.059379
62.368352	2106.669759	20.064397
61.931084	2122.089177	20.069415
62.527674	2114.668366	20.074432
61.916321	2128.007680	20.079450
62.666462	2132.953217	20.084467
62.666896	2143.059911	20.089485
62.817150	2139.332982	20.094503
63.404431	2125.196764	20.099520
63.387046	2151.277391	20.104538
62.994768	2126.701371	20.109555
63.073982	2141.179564	20.114573
63.053377	2152.535470	20.119591
63.448371	2133.270328	20.124608
63.402233	2134.309574	20.129626
63.140051	2140.486218	20.134643
63.210188	2129.514055	20.139661
63.372272	2131.141445	20.144679
63.551065	2123.378266	20.149696
63.382561	2153.006605	20.154714
63.215207	2118.413775	20.159731
63.251790	2142.355884	20.164749
63.430526	2128.552231	20.169767
63.314627	2147.082238	20.174784
63.602501	2119.832132	20.179802
63.350132	2167.496199	20.184819
63.885566	2130.235069	20.189837
63.548521	2176.333335	20.194855
64.010022	2137.160143	20.199872
64.001030	2156.648398	20.204890
64.098141	2153.810845	20.209907
64.091919	2151.950900	20.214925
64.050317	2153.467628	20.219943
63.928835	2160.855109	20.224960
64.364525	2173.041192	20.229978
64.676243	2177.048338	20.234995
64.801890	2178.755478	20.240013
64.720301	2175.925968	20.245031
64.952262	2166.016519	20.250048
64.521126	2170.905054	20.255066
64.707644	2158.791156	20.260083
64.972978	2165.696951	20.265101
65.064175	2175.496608	20.270119
65.172338	2168.167818	20.275136
65.374641	2165.215958	20.280154
65.556011	2168.252871	20.285171
65.417247	2169.969141	20.290189
65.108705	2163.074899	20.295207
65.255668	2159.438153	20.300224
65.207992	2173.832794	20.305242
65.125551	2172.294891	20.310259
65.486889	2144.002680	20.315277
65.402666	2169.666131	20.320295
65.493525	2177.529425	20.325312
65.422311	2158.980399	20.330330
65.432734	2171.103736	20.335347
65.886407	2157.276661	20.340365
65.212928	2166.712185	20.345383
65.582360	2170.260236	20.350400
65.832946	2193.389645	20.355418
65.496927	2201.171587	20.360435
65.929885	2199.129913	20.365453
65.970437	2188.881306	20.370471
65.712817	2195.488261	20.375488
66.010550	2193.737143	20.380506
65.985304	2217.025409	20.385523
66.435932	2233.542914	20.390541
66.300322	2235.379815	20.395559
66.389577	2222.395746	20.400576
66.568872	2212.653542	20.405594
66.397794	2232.701011	20.410611
66.732620	2232.331406	20.415629
66.804139	2221.717608	20.420647
66.909869	2214.401768	20.425664
66.735558	2211.168606	20.430682
66.523647	2224.475768	20.435699
67.035266	2217.192728	20.440717
66.923985	2221.371165	20.445735
66.926665	2239.100572	20.450752
67.336673	2251.010814	20.455770
66.777877	2241.040223	20.460787
67.415255	2256.389083	20.465805
66.916807	2241.964990	20.470823
67.027025	2249.900743	20.475840
67.191012	2226.599682	20.480858
67.024946	2273.355267	20.485875
67.669221	2263.554609	20.490893
67.916389	2257.564300	20.495911
67.785711	2282.554225	20.500928
68.239962	2259.287050	20.505946
68.033675	2279.996163	20.510963
68.260477	2268.110135	20.515981
68.233769	2269.111684	20.520999
68.225902	2285.669331	20.526016
68.439525	2259.448574	20.531034
68.404464	2281.681416	20.536051
68.695579	2255.662244	20.541069
68.548337	2260.417444	20.546087
68.522394	2268.834253	20.551104
68.777646	2271.425243	20.556122
68.267214	2251.874889	20.561139
68.446141	2242.692731	20.566157
68.240669	2264.617663	20.571175
68.444433	2254.558491	20.576192
68.310954	2261.740293	20.581210
68.637155	2256.069295	20.586227
68.565791	2272.048731	20.591245
68.729270	2293.625427	20.596263
68.782090	2288.067228	20.601280
68.976587	2294.501452	20.606298
69.016805	2292.110255	20.611315
69.148116	2291.368827	20.616333
69.187732	2287.439275	20.621351
69.093942	2310.444460	20.626368
69.488373	2295.734778	20.631386
69.647486	2321.477671	20.636403
69.851140	2318.939281	20.641421
70.235693	2299.598505	20.646439
69.496695	2324.960797	20.651456
69.913479	2284.960616	20.656474
69.886471	2315.818876	20.661491
70.178092	2311.090916	20.666509
70.061247	2307.768342	20.671527
70.061698	2303.148167	20.676544
70.313529	2310.927660	20.681562
70.298254	2317.882996	20.686579
70.222820	2292.246262	20.691597
70.296190	2286.181407	20.696615
69.978888	2313.370393	20.701632
70.391110	2303.562669	20.706650
70.216990	2300.033721	20.711667
70.401689	2307.839649	20.716685
70.405484	2314.079346	20.721703
70.266921	2308.131652	20.726720
70.637649	2312.189203	20.731738
70.561635	2336.437458	20.736755
70.861592	2331.333773	20.741773
70.876906	2332.372671	20.746791
70.648233	2342.888856	20.751808
71.071622	2332.093021	20.756826
70.858363	2341.305824	20.761843
71.077381	2335.095024	20.766861
71.148526	2339.754076	20.771879
71.341885	2358.944487	20.776896
71.674751	2360.338598	20.781914
71.137977	2367.205656	20.786931
71.649159	2369.187974	20.791949
71.756399	2374.291177	20.796967
71.890950	2361.293469	20.801984
72.015410	2359.908173	20.807002
71.726094	2361.840388	20.812019
71.840675	2360.720943	20.817037
71.885332	2365.083771	20.822055
71.856107	2366.221011	20.827072
71.744623	2367.025295	20.832090
72.053658	2380.024576	20.837107
71.861503	2370.737915	20.842125
72.019571	2384.591854	20.847143
72.063811	2395.712660	20.852160
72.143171	2380.573350	20.857178
71.918228	2398.911848	20.862195
72.249162	2417.938822	20.867213
72.447602	2418.405813	20.872231
72.795215	2429.317027	20.877248
73.496728	2411.246154	20.882266
73.195659	2413.828355	20.887283
73.060532	2410.021021	20.892301
73.443448	2407.875612	20.897319
73.532370	2408.880754	20.902336
73.523027	2400.722700	20.907354
73.821149	2399.633760	20.912371
73.710523	2401.586250	20.917389
73.687096	2365.758613	20.922407
73.341515	2372.071353	20.927424
73.871100	2368.236683	20.932442
73.647969	2361.772329	20.937459
73.480746	2360.037134	20.942477
73.684739	2371.697177	20.947495
73.358031	2391.071241	20.952512
73.957800	2403.418550	20.957530
74.033605	2399.794666	20.962547
73.938132	2404.516489	20.967565
73.949918	2409.675826	20.972583
73.681060	2398.982468	20.977600
74.080966	2409.077556	20.982618
74.109146	2415.127786	20.987635
74.068576	2408.950485	20.992653
74.231834	2406.368184	20.997671
73.991369	2416.364042	21.002688
74.181546	2430.581004	21.007706
74.796618	2428.323064	21.012723
74.652025	2420.479158	21.017741
74.739113	2425.489636	21.022759
74.651727	2426.533120	21.027776
74.798718	2431.447528	21.032794
74.539600	2441.523459	21.037811
74.559727	2461.000401	21.042829
74.898896	2466.334861	21.047847
74.399348	2471.912400	21.052864
75.019295	2467.170574	21.057882
75.148673	2486.519226	21.062899
75.101638	2482.785917	21.067917
75.384818	2492.089542	21.072935
75.243988	2494.470019	21.077952
75.682101	2473.639418	21.082970
75.844440	2487.156136	21.087987
75.579216	2490.553781	21.093005
75.773729	2504.329661	21.098023
75.974444	2516.061918	21.103040
76.069046	2512.139269	21.108058
76.289359	2506.430003	21.113075
76.415097	2515.368626	21.118093
76.328624	2518.702378	21.123111
76.360558	2521.516223	21.128128
76.708648	2513.342008	21.133146
76.683260	2509.889182	21.138163
76.556385	2515.628326	21.143181
76.979684	2512.347776	21.148199
76.766199	2512.087626	21.153216
76.706977	2503.538693	21.158234
76.894160	2495.342954	21.163251
76.747754	2518.422141	21.168269
77.236402	2487.192469	21.173287
76.780863	2510.616678	21.178304
76.972193	2505.940044	21.183322
77.209589	2491.502967	21.188339
76.787005	2511.553959	21.193357
77.080360	2502.996781	21.198375
77.151050	2515.701487	21.203392
77.292127	2516.102121	21.208410
77.234029	2524.228466	21.213427
77.183209	2532.354441	21.218445
77.241228	2538.527383	21.223463
77.014071	2524.675607	21.228480
77.267978	2540.357279	21.233498
77.390065	2556.054484	21.238515
77.081232	2552.007387	21.243533
77.492746	2564.136307	21.248551
77.347653	2577.872814	21.253568
77.683313	2583.634972	21.258586
78.181257	2598.363040	21.263603
78.325120	2608.022451	21.268621
78.665081	2595.019308	21.273639
78.862994	2615.903551	21.278656
79.046167	2602.761016	21.283674
79.268498	2578.074421	21.288691
79.001097	2584.759405	21.293709
79.101031	2561.733088	21.298727
79.077074	2562.237909	21.303744
79.217064	2577.767895	21.308762
79.127883	2568.048603	21.313779
79.552681	2563.736645	21.318797
79.740348	2565.841371	21.323815
79.494667	2555.543765	21.328832
79.404775	2557.929500	21.333850
79.586275	2568.151554	21.338867
79.417130	2563.191811	21.343885
79.640669	2548.926781	21.348903
79.728444	2549.225800	21.353920
79.719672	2557.355309	21.358938
80.039368	2550.555761	21.363955
79.785849	2560.710321	21.368973
79.803073	2562.533115	21.373991
79.547557	2564.686490	21.379008
79.702413	2560.143075	21.384026
80.097965	2581.765780	21.389043
79.877492	2595.762086	21.394061
80.186356	2598.023676	21.399079
80.354260	2585.964304	21.404096
80.073082	2596.367129	21.409114
80.298530	2603.716815	21.414131
80.197452	2621.825046	21.419149
80.373718	2620.376407	21.424167
80.502933	2615.475252	21.429184
80.274731	2642.405239	21.434202
80.862592	2629.961097	21.439219
80.907054	2645.650327	21.444237
81.205021	2637.472238	21.449255
81.191619	2652.614613	21.454272
81.018249	2652.827070	21.459290
81.185477	2665.073685	21.464307
81.198538	2642.573138	21.469325
81.235849	2642.142425	21.474343
81.090770	2643.598623	21.479360
81.341397	2677.740475	21.484378
81.952891	2654.001625	21.489395
81.699991	2659.535969	21.494413
81.978012	2682.806510	21.499431
82.234121	2651.057478	21.504448
81.937572	2672.490222	21.509466
81.773880	2666.614817	21.514483
81.909144	2662.353719	21.519501
82.002052	2657.327773	21.524519
82.284006	2661.161257	21.529536
82.172253	2674.612527	21.534554
82.710572	2685.782188	21.539571
82.563237	2698.005843	21.544589
82.723873	2688.386640	21.549607
82.782880	2711.446748	21.554624
82.892162	2696.316496	21.559642
83.257110	2698.158580	21.564659
82.681814	2691.026608	21.569677
83.047788	2697.439961	21.574695
82.990424	2699.549173	21.579712
83.125574	2690.560914	21.584730
83.200949	2675.344065	21.589747
83.064523	2702.895848	21.594765
83.210266	2702.364467	21.599783
83.147850	2708.451289	21.604800
83.341463	2721.160169	21.609818
83.750816	2725.565629	21.614835
83.446907	2721.386344	21.619853
83.295954	2723.162827	21.624871
83.620392	2718.995035	21.629888
83.692170	2748.436037	21.634906
83.807095	2734.559399	21.639923
83.728580	2763.813602	21.644941
84.073526	2755.531210	21.649959
84.490663	2755.500059	21.654976
84.141820	2769.161479	21.659994
84.676128	2765.591025	21.665011
84.478754	2778.886148	21.670029
84.893078	2772.089499	21.675047
84.711900	2774.322290	21.680064
84.705060	2774.622244	21.685082
84.959774	2769.500454	21.690099
84.975654	2766.008737	21.695117
84.930731	2767.645614	21.700135
84.921344	2771.804813	21.705152
85.099712	2781.883577	21.710170
85.096705	2804.558084	21.715187
85.157121	2807.106305	21.720205
85.328135	2785.442416	21.725223
85.282481	2804.115434	21.730240
85.528155	2810.242051	21.735258
85.925985	2789.231798	21.740275
86.055977	2796.640851	21.745293
85.929922	2799.898391	21.750311
86.339559	2783.057374	21.755328
86.496303	2787.917649	21.760346
86.353303	2793.567447	21.765363
86.408658	2797.658910	21.770381
86.673542	2796.738060	21.775399
86.727824	2786.524598	21.780416
86.001969	2793.057827	21.785434
86.454753	2779.459984	21.790451
86.743529	2786.450435	21.795469
86.379107	2799.202748	21.800487
86.298219	2797.741612	21.805504
86.405444	2807.787693	21.810522
86.723924	2807.758117	21.815539
86.593238	2820.481042	21.820557
86.583205	2810.915717	21.825575
87.129049	2821.739773	21.830592
86.844173	2848.751541	21.835610
87.179312	2849.213268	21.840627
87.288164	2844.543386	21.845645
87.416602	2845.731032	21.850663
87.669582	2844.469138	21.855680
87.528526	2847.172197	21.860698
87.482536	2851.649519	21.865715
87.720213	2864.998050	21.870733
87.802773	2871.981310	21.875751
88.129620	2875.209907	21.880768
87.465827	2883.273365	21.885786
88.165355	2873.232247	21.890803
88.396009	2869.040827	21.895821
87.914967	2869.780577	21.900839
88.522437	2901.197254	21.905856
88.699206	2905.129378	21.910874
88.883135	2890.862466	21.915891
88.576471	2912.894175	21.920909
88.669017	2901.072303	21.925927
89.460858	2888.411362	21.930944
89.237281	2905.861463	21.935962
89.467988	2901.592156	21.940979
89.634825	2897.294494	21.945997
89.599583	2891.613246	21.951015
89.621539	2877.690732	21.956032
89.750244	2893.181166	21.961050
90.079086	2889.717385	21.966067
89.791847	2867.609676	21.971085
89.688057	2851.831292	21.976103
89.863440	2852.965046	21.981120
89.572643	2875.459812	21.986138
90.060164	2875.418226	21.991155
90.003589	2878.777182	21.996173
89.926328	2888.971507	22.001191
90.016715	2879.197417	22.006208
90.201834	2877.833076	22.011226
90.250886	2870.646289	22.016243
90.240659	2879.752331	22.021261
90.032818	2896.640668	22.026279
90.256221	2903.440240	22.031296
90.146782	2901.120788	22.036314
90.074212	2902.983113	22.041331
90.424308	2917.556534	22.046349
90.311198	2931.828643	22.051367
90.725125	2930.563887	22.056384
90.456346	2928.272199	22.061402
90.643374	2946.074539	22.066419
90.734815	2965.337063	22.071437
91.011023	2971.780585	22.076455
91.450628	2956.119945	22.081472
91.451250	2968.394957	22.086490
91.511346	2973.883441	22.091507
92.116940	2982.436713	22.096525
91.591399	3001.563273	22.101543
92.424374	2980.521900	22.106560
92.240231	2986.005287	22.111578
92.114062	2985.751653	22.116595
92.237493	2985.956115	22.121613
92.078894	2996.850945	22.126631
92.412007	2984.473870	22.131648
92.509838	2990.380303	22.136666
92.545363	2987.759276	22.141683
92.897318	2979.921624	22.146701
92.857991	2981.652808	22.151719
93.123911	2974.281154	22.156736
92.577133	2979.015347	22.161754
92.786133	2973.333662	22.166771
92.953350	2981.944253	22.171789
92.763190	2998.994281	22.176807
93.232669	2989.546658	22.181824
93.216914	3007.029026	22.186842
93.351860	3008.168454	22.191859
93.266878	3005.550909	22.196877
93.208632	3005.313974	22.201895
93.288683	3022.231272	22.206912
93.786878	3037.898913	22.211930
93.814343	3038.912327	22.216947
94.157070	3029.130934	22.221965
94.146844	3030.883440	22.226983
94.516381	3022.145487	22.232000
94.266671	3025.261548	22.237018
94.456232	3022.077939	22.242035
94.454339	3021.008481	22.247053
94.568571	3019.223605	22.252071
94.862313	3013.817849	22.257088
94.819984	3024.998561	22.262106
95.214298	3031.414625	22.267123
94.902612	3016.920644	22.272141
94.650776	3037.961375	22.277159
95.215876	3038.043496	22.282176
94.956701	3053.046140	22.287194
95.103557	3055.749734	22.292211
95.115851	3044.213483	22.297229
95.307486	3052.594477	22.302247
95.465193	3033.956704	22.307264
95.425178	3055.111557	22.312282
95.442668	3076.140073	22.317299
95.837918	3068.886971	22.322317
95.696537	3073.293836	22.327335
95.703220	3088.640330	22.332352
95.981945	3075.356282	22.337370
96.102027	3074.513566	22.342387
96.014323	3068.664422	22.347405
96.033107	3075.479398	22.352423
96.052088	3090.574590	22.357440
96.098672	3110.411578	22.362458
96.508107	3114.755793	22.367475
96.475937	3099.514749	22.372493
96.349422	3114.482144	22.377511
96.747476	3128.719343	22.382528
97.025544	3128.687561	22.387546
96.817439	3141.057353	22.392563
97.213113	3128.267456	22.397581
96.891927	3142.863982	22.402599
97.396759	3123.987470	22.407616
97.312843	3130.779520	22.412634
97.798699	3149.235296	22.417651
98.206087	3153.013516	22.422669
97.956135	3150.358537	22.427687
97.961180	3157.156865	22.432704
98.073293	3156.137649	22.437722
98.002732	3162.300683	22.442739
98.413871	3146.916536	22.447757
98.255544	3153.712596	22.452775
98.758428	3156.177739	22.457792
98.825324	3135.436855	22.462810
98.773969	3145.587113	22.467827
99.057144	3139.049541	22.472845
99.028725	3147.534898	22.477863
99.147642	3133.755567	22.482880
98.997923	3139.762100	22.487898
98.924323	3149.303166	22.492915
99.043871	3145.598184	22.497933
99.064741	3148.027706	22.502951
99.127732	3143.007937	22.507968
99.295778	3136.896170	22.512986
99.083646	3140.656760	22.518003
99.264305	3150.972962	22.523021
99.225215	3165.821854	22.528039
99.484505	3178.319299	22.533056
99.531516	3175.454142	22.538074
99.577353	3189.071895	22.543091
99.817235	3185.634815	22.548109
100.059330	3199.677499	22.553127
99.859480	3208.110781	22.558144
100.089411	3198.919105	22.563162
100.299982	3199.454197	22.568179
100.214364	3202.695152	22.573197
100.439886	3221.016338	22.578215
100.484543	3224.168879	22.583232
100.861009	3227.018379	22.588250
100.375359	3240.797228	22.593267
100.828148	3229.717599	22.598285
101.105964	3227.629739	22.603303
101.137843	3237.888709	22.608320
101.240066	3244.504826	22.613338
101.208603	3275.983296	22.618355
101.576030	3247.189287	22.623373
101.577490	3261.872135	22.628391
101.494035	3254.482899	22.633408
101.748831	3249.286205	22.638426
101.858681	3248.022717	22.643443
101.866905	3248.780429	22.648461
101.966748	3266.357156	22.653479
102.315840	3269.023037	22.658496
102.557776	3266.156670	22.663514
102.211027	3270.446890	22.668531
102.419806	3270.025000	22.673549
102.252629	3274.291307	22.678567
102.653010	3277.677386	22.683584
102.857758	3278.463543	22.688602
102.787449	3283.016453	22.693619
102.969344	3275.535340	22.698637
102.927455	3294.624488	22.703655
103.323776	3289.460274	22.708672
103.504039	3289.355991	22.713690
103.268934	3304.629571	22.718707
103.607289	3288.029812	22.723725
103.796036	3289.776578	22.728743
103.571357	3289.253903	22.733760
103.982798	3288.142900	22.738778
103.938791	3288.382719	22.743795
104.135468	3280.566521	22.748813
103.886590	3283.619576	22.753831
103.826457	3292.360207	22.758848
103.988570	3292.796054	22.763866
104.385423	3313.791165	22.768883
104.627507	3315.608875	22.773901
104.118929	3315.086633	22.778919
104.176549	3324.334731	22.783936
104.683610	3331.536841	22.788954
104.644557	3340.200200	22.793971
104.818445	3348.533067	22.798989
104.833538	3345.011447	22.804007
104.788342	3344.600949	22.809024
105.084924	3360.660558	22.814042
105.119924	3372.320037	22.819059
105.767874	3364.591515	22.824077
105.568540	3362.425548	22.829095
105.601155	3376.474274	22.834112
105.725535	3374.034870	22.839130
105.765813	3371.570335	22.844147
106.085320	3376.183824	22.849165
105.872564	3385.775551	22.854183
106.291679	3398.785727	22.859200
106.415796	3389.392919	22.864218
106.219870	3401.670532	22.869235
106.719731	3387.929328	22.874253
106.873676	3388.491548	22.879271
106.849597	3386.722391	22.884288
106.989651	3380.143820	22.889306
107.116322	3388.941246	22.894323
107.214578	3390.545924	22.899341
107.248998	3384.703136	22.904359
107.175562	3370.704905	22.909376
107.185818	3384.316715	22.914394
107.164359	3384.704751	22.919411
107.448301	3390.513238	22.924429
107.745940	3396.403708	22.929447
107.255858	3404.604143	22.934464
107.303604	3411.658501	22.939482
107.503002	3421.787059	22.944499
107.629974	3417.873165	22.949517
108.003734	3428.530831	22.954535
107.910341	3437.416865	22.959552
108.328813	3430.577565	22.964570
108.462696	3445.606820	22.969587
108.727226	3455.096530	22.974605
109.005199	3465.052125	22.979623
108.975505	3460.758892	22.984640
109.368683	3446.904070	22.989658
109.144799	3474.573511	22.994675
109.268099	3456.618729	22.999693
109.440625	3446.189304	23.004711
109.423158	3467.491399	23.009728
109.877398	3453.034531	23.014746
109.340481	3448.848137	23.019763
109.297090	3460.406916	23.024781
110.047329	3447.242423	23.029799
109.621129	3451.778980	23.034816
109.688623	3448.522714	23.039834
109.759268	3455.199024	23.044851
109.729628	3480.237031	23.049869
110.087043	3491.159285	23.054887
109.945792	3486.766630	23.059904
110.157148	3498.391009	23.064922
110.238810	3512.886698	23.069939
110.575373	3510.059471	23.074957
110.725717	3509.956025	23.079975
110.544968	3521.288190	23.084992
111.074660	3529.779168	23.090010
110.954534	3544.851388	23.095027
111.178402	3548.551999	23.100045
111.426517	3535.123749	23.105063
111.305771	3545.007681	23.110080
111.659823	3540.196223	23.115098
111.604707	3546.233460	23.120115
111.855949	3564.834940	23.125133
112.007163	3562.191431	23.130151
111.794630	3570.205328	23.135168
112.276573	3562.809947	23.140186
112.647085	3563.703411	23.145203
112.369842	3571.715040	23.150221
112.462749	3558.144759	23.155239
112.266148	3566.528960	23.160256
112.806964	3558.176344	23.165274
112.508421	3565.371733	23.170291
112.572274	3566.408485	23.175309
112.714497	3567.583769	23.180327
112.734072	3595.264173	23.185344
113.093182	3595.051139	23.190362
113.223098	3586.686152	23.195379
113.103305	3575.514286	23.200397
113.189324	3607.921803	23.205415
113.335500	3619.041449	23.210432
113.626237	3618.251725	23.215450
113.778509	3627.488857	23.220467
113.604506	3635.948155	23.225485
113.899198	3620.587586	23.230503
114.152024	3625.767129	23.235520
114.552782	3644.571412	23.240538
114.807115	3656.048263	23.245555
114.759182	3656.103075	23.250573
114.714076	3643.294127	23.255591
114.740446	3634.944050	23.260608
114.795644	3636.839584	23.265626
114.972905	3646.210398	23.270643
115.005844	3647.516385	23.275661
114.995952	3619.347376	23.280679
115.265183	3656.050518	23.285696
115.196627	3653.035361	23.290714
115.722388	3673.639162	23.295731
115.678287	3674.015870	23.300749
115.951252	3658.491180	23.305767
115.714661	3684.563094	23.310784
115.946575	3655.250281	23.315802
115.974275	3668.171297	23.320819
115.844977	3687.328385	23.325837
116.456157	3671.660866	23.330855
116.268329	3693.707837	23.335872
116.298823	3691.365159	23.340890
116.368636	3688.276016	23.345907
116.428922	3702.074436	23.350925
116.727197	3715.613100	23.355943
116.571167	3725.022162	23.360960
116.848355	3730.065708	23.365978
117.053219	3720.905234	23.370995
116.895517	3732.848227	23.376013
117.230159	3740.310085	23.381031
117.236119	3746.951220	23.386048
117.112423	3751.491550	23.391066
117.670338	3766.287550	23.396083
117.598917	3782.318204	23.401101
117.956881	3770.379368	23.406119
117.755871	3775.628182	23.411136
118.316327	3779.223268	23.416154
118.597609	3791.551760	23.421171
118.367865	3810.919318	23.426189
118.853363	3790.821068	23.431207
118.740522	3793.619700	23.436224
119.154564	3797.220830	23.441242
119.381034	3792.098471	23.446259
119.176451	3794.177037	23.451277
119.266246	3791.456753	23.456295
119.015056	3797.968219	23.461312
119.199671	3793.753989	23.466330
119.427900	3781.063380	23.471347
119.275748	3798.076026	23.476365
119.619036	3804.704304	23.481383
119.576192	3817.880550	23.486400
119.623620	3822.973349	23.491418
119.744472	3825.899913	23.496435
119.783126	3829.578999	23.501453
119.903491	3849.177896	23.506471
119.633718	3851.976389	23.511488
119.877480	3856.198579	23.516506
120.366574	3882.137042	23.521523
120.285628	3884.408293	23.526541
120.561204	3887.003418	23.531559
120.495124	3893.714316	23.536576
120.679173	3908.746276	23.541594
120.912072	3908.594267	23.546611
120.982420	3926.760949	23.551629
121.645132	3924.975040	23.556647
121.731999	3938.949580	23.561664
121.758371	3945.305942	23.566682
122.123587	3934.654298	23.571699
122.061974	3944.400851	23.576717
122.344482	3938.950926	23.581735
122.591144	3941.237598	23.586752
122.663513	3930.605119	23.591770
122.945009	3927.915600	23.596787
122.986016	3935.385047	23.601805
123.143890	3926.347570	23.606823
123.170724	3932.002976	23.611840
123.082131	3921.344252	23.616858
123.159764	3924.798467	23.621875
123.052913	3925.870331	23.626893
123.163217	3919.043759	23.631911
123.488550	3935.734220	23.636928
123.459115	3951.880290	23.641946
123.497185	3949.092710	23.646963
123.533245	3954.251870	23.651981
123.437051	3939.176695	23.656999
123.957732	3960.175808	23.662016
123.885710	3983.240726	23.667034
124.167049	3967.310839	23.672051
124.220627	3966.765794	23.677069
124.250466	3970.321249	23.682087
124.576548	3974.848142	23.687104
124.627659	3992.749736	23.692122
124.692809	4000.410448	23.697139
124.664707	4008.409335	23.702157
124.882533	4006.592878	23.707175
124.873716	4003.755340	23.712192
125.099409	4015.758571	23.717210
125.559938	4028.628199	23.722227
125.577986	4042.694047	23.727245
125.776603	4029.535971	23.732263
126.010840	4029.823471	23.737280
125.872183	4028.827662	23.742298
125.906303	4018.542612	23.747315
125.905362	4029.512971	23.752333
126.227248	4045.308145	23.757351
126.267934	4049.587943	23.762368
126.295570	4057.708548	23.767386
126.599883	4044.972542	23.772403
126.770272	4048.847787	23.777421
126.992984	4051.889522	23.782439
126.913979	4064.696536	23.787456
126.981873	4073.104929	23.792474
127.571913	4079.740402	23.797491
127.507771	4084.735448	23.802509
127.670694	4076.634732	23.807527
127.864723	4075.335728	23.812544
127.587212	4089.833407	23.817562
128.089348	4075.221195	23.822579
127.671566	4091.427766	23.827597
127.799570	4106.817341	23.832615
127.953450	4102.614217	23.837632
128.236580	4102.369243	23.842650
128.328522	4112.339211	23.847667
128.481281	4119.639902	23.852685
128.728941	4126.562042	23.857703
128.979349	4124.417859	23.862720
129.057715	4131.670633	23.867738
129.471885	4121.645071	23.872755
129.279094	4121.767819	23.877773
129.443023	4137.887196	23.882791
129.726753	4139.189425	23.887808
129.714605	4157.333362	23.892826
129.894153	4142.433481	23.897843
130.119346	4151.531098	23.902861
130.059769	4131.221948	23.907879
130.313022	4132.126282	23.912896
129.993849	4147.227711	23.917914
130.182904	4155.922046	23.922931
130.056840	4155.451261	23.927949
130.211431	4177.139936	23.932967
130.670404	4176.460236	23.937984
130.885473	4187.415938	23.943002
131.188715	4192.254901	23.948019
131.065333	4192.622237	23.953037
131.477769	4197.492563	23.958055
131.877006	4194.170652	23.963072
131.194627	4214.120647	23.968090
131.698146	4198.660103	23.973107
131.681638	4198.894764	23.978125
131.760939	4207.184208	23.983143
131.829211	4219.927756	23.988160
132.040870	4234.826643	23.993178
132.352470	4219.652333	23.998195
132.177418	4235.791255	24.003213
132.175841	4242.822414	24.008231
132.652469	4246.047109	24.013248
132.552623	4259.782698	24.018266
132.827142	4250.536059	24.023283
132.954208	4256.324283	24.028301
132.910859	4270.260905	24.033319
133.355124	4272.268334	24.038336
133.508464	4277.472627	24.043354
133.988472	4274.357291	24.048371
133.819399	4269.177479	24.053389
133.975478	4270.231830	24.058407
134.394751	4258.628944	24.063424
133.955665	4276.439917	24.068442
134.161076	4291.004750	24.073459
134.287714	4292.541286	24.078477
134.322641	4301.874646	24.083495
134.515009	4293.300280	24.088512
134.676131	4307.555177	24.093530
134.669413	4308.891931	24.098547
134.814479	4327.859795	24.103565
134.945613	4328.713602	24.108583
135.472064	4320.204737	24.113600
135.046459	4347.003351	24.118618
135.571166	4347.267358	24.123635
135.783974	4350.630112	24.128653
135.944733	4355.630296	24.133671
135.869296	4349.539543	24.138688
135.859621	4365.162162	24.143706
136.215922	4376.657936	24.148723
136.258572	4389.000597	24.153741
136.579699	4387.599491	24.158759
136.863965	4383.210303	24.163776
136.680835	4401.774339	24.168794
136.703478	4396.625272	24.173811
136.815325	4393.607157	24.178829
137.083315	4407.750715	24.183847
137.560037	4403.505471	24.188864
137.336250	4422.378872	24.193882
137.983411	4403.830448	24.198899
138.035172	4407.273170	24.203917
137.969820	4422.674241	24.208935
138.331347	4433.617004	24.213952
137.838705	4434.487674	24.218970
138.690210	4434.849828	24.223987
138.517676	4434.904842	24.229005
138.360645	4429.856782	24.234023
138.620962	4424.985255	24.239040
138.457659	4435.571177	24.244058
138.754688	4440.043852	24.249075
138.557462	4457.897505	24.254093
138.956432	4459.916904	24.259111
139.190062	4451.351601	24.264128
139.418278	4473.055722	24.269146
139.566632	4480.923681	24.274163
139.826719	4481.307762	24.279181
140.071509	4481.578644	24.284199
140.114448	4470.195285	24.289216
139.977302	4479.144777	24.294234
140.383859	4477.031500	24.299251
140.535298	4485.128671	24.304269
140.719787	4482.377429	24.309287
140.724515	4482.307423	24.314304
140.818574	4497.665064	24.319322
140.499612	4498.924969	24.324339
140.651075	4493.503602	24.329357
140.785494	4507.776325	24.334375
141.142895	4516.400768	24.339392
140.982920	4536.647857	24.344410
141.385175	4520.216664	24.349427
141.636744	4538.415784	24.354445
141.590223	4563.284484	24.359463
141.678259	4554.671536	24.364480
141.920607	4578.261522	24.369498
142.181844	4590.394864	24.374515
142.385566	4594.057264	24.379533
142.538875	4593.195795	24.384551
142.859558	4588.812540	24.389568
143.062419	4599.909737	24.394586
143.477645	4604.289672	24.399603
143.461961	4610.629428	24.404621
143.601533	4607.292188	24.409639
143.830856	4602.814937	24.414656
143.790590	4607.171524	24.419674
143.781016	4606.705751	24.424691
144.196825	4601.624511	24.429709
144.076763	4610.428188	24.434727
144.238105	4598.623872	24.439744
144.368530	4617.728964	24.444762
144.474245	4614.204390	24.449779
144.468345	4625.334103	24.454797
144.226113	4629.232812	24.459815
144.900868	4631.445835	24.464832
144.841786	4653.280202	24.469850
144.750075	4663.257801	24.474867
145.096308	4661.851095	24.479885
145.365587	4682.649831	24.484903
145.634873	4693.631883	24.489920
145.794669	4698.884070	24.494938
145.820681	4694.760951	24.499955
146.049187	4695.205139	24.504973
145.648475	4695.267427	24.509991
146.172364	4706.643130	24.515008
146.083962	4718.962124	24.520026
146.122840	4729.669421	24.525043
146.569959	4720.066146	24.530061
146.487136	4745.996640	24.535079
146.637847	4750.306301	24.540096
146.619193	4748.886177	24.545114
147.014727	4757.375672	24.550131
147.466708	4756.347788	24.555149
147.475432	4772.288865	24.560167
147.882529	4768.166326	24.565184
148.050904	4769.006355	24.570202
147.683861	4773.212133	24.575219
147.941815	4792.790358	24.580237
148.191457	4801.671297	24.585255
148.575742	4795.337928	24.590272
148.759967	4801.585321	24.595290
148.803574	4796.549198	24.600307
149.118190	4786.670433	24.605325
148.919292	4807.035020	24.610343
149.160964	4816.959570	24.615360
149.303020	4807.417464	24.620378
149.237265	4817.291909	24.625395
149.647879	4817.656721	24.630413
149.590538	4829.493349	24.635431
149.801841	4846.205394	24.640448
149.883634	4849.511272	24.645466
150.104982	4855.907742	24.650483
150.044629	4847.791069	24.655501
150.080199	4874.546220	24.660519
150.718360	4875.860450	24.665536
150.889721	4868.502929	24.670554
150.751749	4881.139909	24.675571
151.327135	4897.886005	24.680589
151.349285	4909.424463	24.685607
151.545596	4909.625991	24.690624
151.500552	4905.281288	24.695642
151.649659	4899.770467	24.700659
151.730107	4902.664357	24.705677
151.686043	4921.354770	24.710695
151.968945	4916.630522	24.715712
152.453836	4927.061532	24.720730
152.371658	4923.814643	24.725747
152.482426	4931.032754	24.730765
152.572491	4946.326994	24.735783
152.515404	4952.874100	24.740800
152.872783	4957.904505	24.745818
153.022602	4979.514101	24.750835
153.412606	4974.345596	24.755853
153.277570	4989.885812	24.760871
152.984911	4997.833016	24.765888
153.800616	4992.517966	24.770906
153.687297	5003.350422	24.775923
154.043988	5014.332153	24.780941
153.927520	5021.354469	24.785959
154.317956	5027.794857	24.790976
154.642280	5025.294985	24.795994
154.321783	5038.636955	24.801011
155.108408	5035.713304	24.806029
155.165386	5032.487471	24.811047
155.053729	5038.348680	24.816064
155.166195	5031.964934	24.821082
155.217590	5044.553768	24.826099
155.593878	5057.724877	24.831117
155.726226	5076.387361	24.836135
156.000813	5079.371482	24.841152
155.710847	5061.159662	24.846170
155.701654	5087.087672	24.851187
156.217610	5084.800322	24.856205
156.320074	5094.799176	24.861223
156.504365	5108.319547	24.866240
156.757326	5098.711583	24.871258
156.861076	5115.343534	24.876275
156.592778	5123.146892	24.881293
156.816441	5128.505480	24.886311
157.349379	5137.274589	24.891328
157.636085	5148.874899	24.896346
157.546299	5149.792298	24.901363
157.710248	5146.323608	24.906381
158.137665	5158.050173	24.911399
158.212114	5165.135734	24.916416
158.824788	5170.798125	24.921434
158.536338	5178.478855	24.926451
158.869109	5168.101332	24.931469
158.867363	5160.676863	24.936487
158.975103	5166.362327	24.941504
159.203646	5177.820103	24.946522
159.276900	5186.716812	24.951539
159.760656	5192.781308	24.956557
159.529926	5182.887743	24.961575
159.741477	5209.057688	24.966592
160.109010	5187.699557	24.971610
160.083218	5189.735648	24.976627
160.286422	5226.102394	24.981645
160.313185	5225.749597	24.986663
160.418071	5206.337096	24.991680
160.406647	5236.870985	24.996698
160.512259	5242.104473	25.001715
160.893455	5250.315695	25.006733
160.975569	5245.790133	25.011751
160.820892	5257.976179	25.016768
161.256345	5286.967819	25.021786
161.376893	5285.511289	25.026803
161.333307	5294.890839	25.031821
161.998416	5305.727642	25.036839
161.707896	5304.272926	25.041856
162.064769	5311.335558	25.046874
162.286698	5335.274589	25.051891
162.792686	5344.452481	25.056909
163.055102	5334.022336	25.061927
162.806086	5340.791380	25.066944
163.180874	5337.879051	25.071962
163.240024	5335.045366	25.076979
163.175473	5339.409188	25.081997
163.447442	5337.801069	25.087015
163.299024	5363.795031	25.092032
163.797634	5362.088626	25.097050
163.939203	5353.306978	25.102067
164.064332	5397.633778	25.107085
164.299266	5379.804388	25.112103
163.997969	5405.705579	25.117120
164.562459	5381.427805	25.122138
164.508062	5397.378837	25.127155
164.589537	5404.858315	25.132173
164.708807	5424.959834	25.137191
165.231145	5427.771577	25.142208
165.581788	5430.801076	25.147226
165.267276	5463.233281	25.152243
165.684202	5438.173360	25.157261
165.708284	5450.467952	25.162279
165.655211	5460.733369	25.167296
166.182657	5460.715334	25.172314
166.084486	5486.589004	25.177331
166.828903	5474.160793	25.182349
166.669024	5490.540186	25.187367
167.005222	5506.878270	25.192384
167.499932	5482.904108	25.197402
167.281631	5498.294501	25.202419
167.422391	5495.649170	25.207437
167.477102	5522.839855	25.212455
167.718517	5512.365731	25.217472
167.759338	5523.820664	25.222490
168.013454	5538.242874	25.227507
168.378636	5531.515742	25.232525
168.565864	5559.007129	25.237543
168.660065	5552.114713	25.242560
168.651405	5544.129446	25.247578
168.624280	5553.088796	25.252595
169.168835	5577.436221	25.257613
169.777748	5558.224542	25.262631
169.331051	5578.805134	25.267648
169.454682	5588.629448	25.272666
169.498645	5578.157649	25.277683
169.678207	5590.290682	25.282701
170.053379	5613.801369	25.287719
170.043737	5609.758416	25.292736
170.243096	5622.549941	25.297754
170.448526	5646.987736	25.302771
170.477122	5641.410102	25.307789
170.562547	5634.327876	25.312807
170.734836	5674.649938	25.317824
171.331686	5666.370606	25.322842
171.275520	5670.283190	25.327859
171.841684	5682.752741	25.332877
171.635276	5704.637329	25.337895
171.659952	5685.379380	25.342912
171.860357	5705.174116	25.347930
171.781413	5708.040868	25.352947
172.008537	5718.006898	25.357965
172.501939	5710.754174	25.362983
172.267259	5714.165772	25.368000
172.503903	5752.622718	25.373018
172.841924	5742.927612	25.378035
173.001738	5754.335432	25.383053
173.347995	5783.661679	25.388071
172.986780	5771.571552	25.393088
173.698995	5794.507202	25.398106
173.820334	5790.643144	25.403123
173.512716	5804.019150	25.408141
174.173610	5807.850495	25.413159
174.093281	5816.492786	25.418176
174.439256	5829.084105	25.423194
175.048445	5848.728898	25.428211
175.082259	5837.698388	25.433229
175.018108	5852.482401	25.438247
175.000360	5834.968886	25.443264
175.657576	5849.289375	25.448282
175.852481	5863.940054	25.453299
175.856161	5876.495511	25.458317
176.396098	5853.935932	25.463335
176.370203	5836.505533	25.468352
176.277620	5879.652223	25.473370
176.697633	5868.360293	25.478387
176.788161	5892.790853	25.483405
177.245611	5893.444042	25.488423
177.082164	5884.557295	25.493440
177.156184	5910.703211	25.498458
177.172991	5888.655744	25.503475
177.313782	5887.204583	25.508493
177.761231	5936.120918	25.513511
177.559928	5956.386771	25.518528
177.714047	5953.135811	25.523546
178.118080	5935.408604	25.528563
178.168199	5973.244454	25.533581
178.642556	5989.980376	25.538599
178.529452	5973.480256	25.543616
178.895498	5988.787441	25.548634
179.023229	5997.317207	25.553651
178.942827	5991.351653	25.558669
179.396557	6012.368328	25.563687
179.070772	6011.558770	25.568704
179.687099	6032.684870	25.573722
180.178753	6040.387223	25.578739
180.165881	6042.463069	25.583757
180.456420	6061.821441	25.588775
180.451655	6065.102057	25.593792
180.682024	6081.209832	25.598810
181.205885	6079.359288	25.603827
181.283486	6091.501123	25.608845
181.615610	6090.774704	25.613863
181.929163	6085.079094	25.618880
181.639325	6086.201524	25.623898
182.153685	6085.265104	25.628915
182.056847	6098.067287	25.633933
182.065570	6071.101393	25.638951
182.220945	6090.478992	25.643968
182.204914	6102.245543	25.648986
182.726302	6106.603507	25.654003
182.262762	6107.268215	25.659021
182.854715	6128.559620	25.664039
183.014338	6135.373234	25.669056
183.103243	6131.615747	25.674074
183.338668	6165.821663	25.679092
183.489080	6157.160860	25.684109
183.818281	6179.266015	25.689127
184.100976	6166.378219	25.694144
184.120255	6201.897125	25.699162
184.956098	6187.216264	25.704180
184.493050	6203.064164	25.709197
184.746735	6194.892749	25.714215
185.029453	6206.497679	25.719232
185.177437	6219.912358	25.724250
185.190738	6228.928612	25.729268
185.128123	6229.115583	25.734285
185.338144	6251.542742	25.739303
185.419065	6241.489422	25.744320
185.324376	6276.785933	25.749338
185.813078	6276.731599	25.754356
186.029887	6297.459167	25.759373
186.472662	6308.135479	25.764391
186.804892	6318.305450	25.769408
186.571525	6307.424968	25.774426
187.203611	6342.744241	25.779444
187.396161	6337.690929	25.784461
187.475001	6323.435087	25.789479
187.356408	6358.158920	25.794496
187.680117	6367.754384	25.799514
188.264590	6356.273011	25.804532
188.282145	6378.465125	25.809549
188.640743	6403.873421	25.814567
188.992311	6384.752054	25.819584
189.221500	6405.125338	25.824602
189.483752	6390.119530	25.829620
189.183235	6414.754122	25.834637
189.394262	6413.593826	25.839655
190.196188	6402.526986	25.844672
190.085151	6428.251726	25.849690
190.402037	6401.594073	25.854708
190.369150	6442.577983	25.859725
190.439256	6403.542371	25.864743
190.731004	6459.122286	25.869760
190.319306	6458.452277	25.874778
190.978178	6458.120628	25.879796
190.534446	6461.837938	25.884813
190.782179	6472.512421	25.889831
190.947643	6503.601355	25.894848
191.007314	6499.997918	25.899866
191.283136	6522.072760	25.904884
191.943528	6520.672454	25.909901
192.014616	6562.314369	25.914919
192.573787	6532.787888	25.919936
192.411069	6557.101781	25.924954
192.914535	6562.926111	25.929972
193.124652	6584.000536	25.934989
193.277920	6571.030744	25.940007
193.205079	6592.837130	25.945024
193.249542	6573.035153	25.950042
193.782588	6583.100126	25.955060
193.601580	6609.371330	25.960077
194.224792	6603.003832	25.965095
194.160860	6602.728402	25.970112
194.437602	6646.720867	25.975130
194.619081	6620.440812	25.980148
194.848046	6649.753651	25.985165
195.116088	6633.350171	25.990183
195.032028	6678.285355	25.995200
195.035345	6650.925097	26.000218
195.270702	6674.232394	26.005236
195.504060	6688.307359	26.010253
195.808148	6709.267850	26.015271
196.325552	6713.614832	26.020288
196.174613	6724.981678	26.025306
196.878931	6702.441029	26.030324
196.805620	6715.146369	26.035341
196.874247	6745.806727	26.040359
197.307453	6713.397583	26.045376
196.904958	6769.880826	26.050394
197.500321	6751.773607	26.055412
197.630612	6765.038969	26.060429
197.793683	6780.146452	26.065447
197.976588	6804.447351	26.070464
198.564894	6801.945233	26.075482
198.780310	6785.573578	26.080500
199.086858	6800.366318	26.085517
199.441988	6813.907442	26.090535
199.517176	6823.590817	26.095552
199.680615	6803.805756	26.100570
200.079340	6812.617732	26.105588
200.211502	6820.599676	26.110605
199.911732	6796.236287	26.115623
200.442284	6811.348163	26.120640
200.140596	6861.022700	26.125658
200.781352	6824.442584	26.130676
200.518648	6850.614731	26.135693
200.806865	6844.131379	26.140711
200.833026	6879.043424	26.145728
200.857232	6859.276552	26.150746
201.536920	6912.111068	26.155764
201.547094	6887.848392	26.160781
201.745374	6920.749637	26.165799
201.440328	6904.375848	26.170816
201.721807	6954.707532	26.175834
202.126800	6946.673661	26.180852
201.946383	6975.714094	26.185869
202.500265	6978.792560	26.190887
202.708486	6985.594887	26.195904
202.799338	7012.021735	26.200922
203.230713	7016.756245	26.205940
203.506499	7018.078894	26.210957
203.641246	7041.773384	26.215975
203.583576	7054.077622	26.220992
203.822873	7061.631130	26.226010
204.119090	7078.603616	26.231028
203.997882	7082.929775	26.236045
204.408639	7118.910899	26.241063
204.951154	7109.794429	26.246080
204.909246	7137.462971	26.251098
205.371325	7122.669261	26.256116
205.924973	7162.918856	26.261133
206.306233	7150.391369	26.266151
206.518015	7148.130180	26.271168
206.513689	7153.196192	26.276186
206.890171	7138.098249	26.281204
206.924202	7162.315679	26.286221
206.927047	7155.290739	26.291239
207.491988	7168.628011	26.296256
207.129289	7159.865098	26.301274
207.515444	7195.117043	26.306292
207.970128	7180.503056	26.311309
207.871421	7207.150874	26.316327
207.952934	7192.541288	26.321344
208.310258	7222.420174	26.326362
208.595372	7230.477094	26.331380
208.742872	7250.801622	26.336397
208.473633	7250.057720	26.341415
209.134945	7226.547512	26.346432
209.023708	7289.348312	26.351450
209.250511	7283.957979	26.356468
209.717026	7295.582464	26.361485
209.654218	7323.027299	26.366503
210.519689	7310.311552	26.371520
210.602339	7323.418995	26.376538
210.593165	7359.134830	26.381556
210.473815	7359.410325	26.386573
210.867424	7350.267878	26.391591
211.357901	7357.484874	26.396608
211.379219	7399.741339	26.401626
211.257649	7377.622445	26.406644
211.811618	7399.027964	26.411661
212.445706	7393.488479	26.416679
212.631652	7387.458657	26.421696
212.760407	7404.302426	26.426714
213.445205	7415.152616	26.431732
213.448629	7425.648003	26.436749
213.427421	7421.950231	26.441767
213.810701	7416.206023	26.446784
213.875960	7423.776445	26.451802
214.164317	7417.126808	26.456820
213.950535	7431.688406	26.461837
213.744381	7426.108181	26.466855
214.104888	7446.284936	26.471872
214.400787	7452.738324	26.476890
214.408714	7452.732312	26.481908
214.505104	7479.368400	26.486925
214.115521	7507.627296	26.491943
215.041638	7511.006112	26.496960
215.293172	7515.995268	26.501978
215.663362	7548.492048	26.506996
215.887425	7537.459059	26.512013
216.156731	7551.094010	26.517031
216.601085	7565.669634	26.522048
216.779646	7592.916769	26.527066
217.255723	7558.204607	26.532084
217.219485	7599.356691	26.537101
217.449954	7590.886864	26.542119
217.655565	7620.081033	26.547136
217.548513	7596.807601	26.552154
217.799249	7636.131909	26.557172
218.031075	7640.326419	26.562189
218.329042	7626.488389	26.567207
218.581986	7672.282418	26.572224
218.765440	7635.696102	26.577242
218.873493	7683.917771	26.582260
218.854958	7697.020430	26.587277
219.183678	7685.654346	26.592295
219.679636	7723.865791	26.597312
220.089750	7713.064238	26.602330
219.925019	7747.740451	26.607348
220.314572	7731.295936	26.612365
220.701752	7766.284705	26.617383
220.976724	7748.045599	26.622400
221.123441	7790.432682	26.627418
221.128262	7773.053332	26.632436
221.536452	7782.347491	26.637453
221.424833	7813.824038	26.642471
221.608739	7807.225499	26.647488
222.007626	7813.443891	26.652506
221.917786	7849.947999	26.657524
222.500078	7830.965036	26.662541
222.817960	7871.605853	26.667559
223.146143	7870.879987	26.672576
223.134289	7876.313320	26.677594
223.373472	7892.681320	26.682612
223.453009	7889.666076	26.687629
223.515391	7912.642529	26.692647
223.710250	7936.063703	26.697664
224.222387	7939.978354	26.702682
224.129674	7956.300189	26.707700
224.656686	7957.304342	26.712717
224.852019	7976.330262	26.717735
224.953547	7993.969020	26.722752
225.410128	8001.107547	26.727770
225.427170	8006.917149	26.732788
226.338310	8007.352567	26.737805
226.174244	8012.798410	26.742823
226.287301	8028.915994	26.747840
226.535842	8022.528945	26.752858
226.776919	8026.223237	26.757876
226.873416	8049.034735	26.762893
227.139224	8037.338500	26.767911
227.102167	8057.651851	26.772928
227.818119	8077.842837	26.777946
227.715139	8088.863951	26.782964
228.107890	8078.647951	26.787981
228.205037	8096.795041	26.792999
228.791294	8098.834684	26.798016
228.693161	8103.738147	26.803034
228.626009	8110.767436	26.808052
229.045471	8110.378728	26.813069
229.334499	8142.016354	26.818087
229.361402	8151.286938	26.823104
229.552321	8167.199485	26.828122
229.582938	8192.922009	26.833140
230.395874	8193.765724	26.838157
230.407689	8202.590638	26.843175
230.833753	8215.515085	26.848192
230.996189	8218.158146	26.853210
231.038465	8244.618536	26.858228
231.346310	8264.927549	26.863245
231.626275	8264.916729	26.868263
232.016478	8264.712870	26.873280
231.960032	8280.052800	26.878298
232.210712	8313.375252	26.883316
232.759309	8293.992634	26.888333
233.040550	8315.361123	26.893351
233.402875	8335.323203	26.898368
233.612475	8332.754528	26.903386
233.618490	8338.099414	26.908404
233.994884	8345.334297	26.913421
234.015450	8376.474647	26.918439
234.650296	8376.086223	26.923456
234.723650	8370.181754	26.928474
234.286720	8398.939305	26.933492
235.051353	8398.183189	26.938509
235.252064	8410.313596	26.943527
235.179465	8429.271858	26.948544
235.503625	8439.597232	26.953562
235.387600	8456.880150	26.958580
235.824891	8461.406459	26.963597
236.164211	8474.526724	26.968615
236.108362	8487.733597	26.973632
236.973582	8503.882091	26.978650
236.968755	8544.056857	26.983668
237.665196	8509.249134	26.988685
237.600509	8519.896997	26.993703
238.044411	8534.047171	26.998720
238.381570	8550.449852	27.003738
238.466864	8553.447555	27.008756
238.298751	8545.371993	27.013773
238.666389	8551.173135	27.018791
238.902008	8568.080664	27.023808
239.206974	8571.925430	27.028826
238.991725	8578.836123	27.033844
239.589157	8588.553074	27.038861
239.419440	8600.081715	27.043879
239.880656	8614.997188	27.048896
240.054849	8620.700933	27.053914
240.063712	8643.813730	27.058932
240.566315	8652.457600	27.063949
240.747926	8666.552138	27.068967
240.901953	8684.409178	27.073984
241.046871	8689.078947	27.079002
241.395038	8734.207965	27.084020
241.635229	8724.566656	27.089037
241.764166	8739.956983	27.094055
241.577323	8766.388722	27.099072
242.488254	8800.437962	27.104090
242.405226	8787.347320	27.109108
242.702791	8830.635537	27.114125
242.850837	8841.610111	27.119143
243.292910	8859.786559	27.124160
243.553489	8864.651978	27.129178
243.433015	8907.069877	27.134196
244.405469	8890.862457	27.139213
244.713444	8914.705435	27.144231
244.641405	8932.808118	27.149248
245.130608	8939.699542	27.154266
245.396422	8947.681002	27.159284
245.574418	8950.087222	27.164301
245.714839	8982.435698	27.169319
246.017603	8985.961448	27.174336
246.676706	8993.075653	27.179354
246.406257	9005.085711	27.184372
246.738367	9024.266252	27.189389
247.076966	9022.573952	27.194407
247.595578	9043.810438	27.199424
247.808037	9032.038128	27.204442
248.184188	9055.652891	27.209460
248.551542	9060.700439	27.214477
248.614200	9064.879041	27.219495
249.147190	9059.432974	27.224512
249.233077	9063.995811	27.229530
248.934303	9087.016689	27.234548
249.324801	9081.538245	27.239565
249.887528	9085.022189	27.244583
249.996516	9111.021413	27.249600
250.113127	9114.428931	27.254618
250.123627	9125.248980	27.259636
250.425850	9139.425857	27.264653
250.552177	9147.742842	27.269671
250.854046	9156.322609	27.274688
251.302727	9168.209910	27.279706
251.201118	9186.942802	27.284724
251.141750	9196.885634	27.289741
251.655242	9208.727226	27.294759
251.627068	9225.388756	27.299776
252.077832	9243.940821	27.304794
251.891612	9265.727093	27.309812
252.226854	9275.275792	27.314829
252.296893	9303.854334	27.319847
252.660067	9339.791767	27.324864
253.185242	9326.581282	27.329882
253.369165	9374.007846	27.334900
253.521117	9388.900996	27.339917
254.054889	9409.292809	27.344935
254.338581	9422.115098	27.349952
254.982276	9433.009531	27.354970
254.901793	9439.359318	27.359988
255.156763	9461.349002	27.365005
255.764090	9475.821448	27.370023
255.622179	9491.812067	27.375040
256.407565	9501.521697	27.380058
256.170703	9525.186123	27.385076
256.494313	9533.973929	27.390093
257.159687	9537.803604	27.395111
256.887503	9560.998419	27.400128
257.210156	9561.422261	27.405146
257.444762	9577.465095	27.410164
257.683189	9588.945178	27.415181
258.449969	9612.142479	27.420199
258.268889	9631.034959	27.425216
258.742391	9637.257184	27.430234
258.839438	9667.864731	27.435252
258.997872	9671.719765	27.440269
259.656734	9679.300987	27.445287
259.719541	9699.213878	27.450304
259.987546	9718.645542	27.455322
260.265689	9720.263954	27.460340
260.603677	9736.730371	27.465357
260.996567	9755.902953	27.470375
260.684384	9762.390139	27.475392
261.076410	9776.736662	27.480410
261.424649	9787.490374	27.485428
262.015541	9807.276744	27.490445
262.437884	9801.462849	27.495463
262.582712	9828.392084	27.500480
263.066586	9832.421137	27.505498
263.356523	9832.130555	27.510516
263.565136	9842.174716	27.515533
263.640373	9860.435252	27.520551
263.740548	9872.813839	27.525568
264.112053	9875.321967	27.530586
264.550981	9894.695927	27.535604
264.367474	9908.665297	27.540621
264.855593	9909.953195	27.545639
264.898620	9929.163664	27.550656
265.131511	9931.874890	27.555674
265.203295	9941.871676	27.560692
265.617131	9967.367769	27.565709
266.061464	9972.425789	27.570727
265.937411	9984.656457	27.575744
266.670856	10003.220285	27.580762
266.641680	10009.126170	27.585780
266.380157	10039.452457	27.590797
267.110919	10043.679480	27.595815
266.993849	10076.004864	27.600832
267.043474	10090.128472	27.605850
267.507204	10094.028208	27.610868
267.621945	10132.196421	27.615885
267.798411	10152.920454	27.620903
267.762988	10180.562515	27.625920
268.379402	10186.266022	27.630938
268.968841	10218.123009	27.635956
269.399893	10234.732533	27.640973
269.935835	10258.074658	27.645991
270.099415	10270.105471	27.651008
270.838893	10279.564025	27.656026
271.187598	10277.382462	27.661044
271.224344	10287.708108	27.666061
271.682140	10298.165752	27.671079
271.627094	10315.045252	27.676096
272.051127	10315.306195	27.681114
272.149072	10340.890652	27.686132
272.291567	10351.740914	27.691149
272.927373	10351.413299	27.696167
272.879117	10382.545576	27.701184
273.065852	10387.720737	27.706202
273.444381	10417.667974	27.711220
273.512622	10428.132317	27.716237
274.227853	10428.957533	27.721255
273.940210	10447.298262	27.726272
274.449407	10463.335661	27.731290
274.780262	10478.396941	27.736308
274.986591	10520.154661	27.741325
275.438054	10510.778373	27.746343
275.470161	10525.681131	27.751360
276.034142	10551.983753	27.756378
276.300897	10554.956479	27.761396
276.178433	10568.447305	27.766413
276.566895	10596.858333	27.771431
276.559310	10609.315693	27.776448
276.995328	10619.668039	27.781466
277.445109	10639.848668	27.786484
277.328921	10664.689096	27.791501
277.947208	10673.762320	27.796519
278.429916	10701.735134	27.801536
278.625269	10711.046956	27.806554
278.882855	10729.147666	27.811572
279.068783	10729.425714	27.816589
279.479139	10771.309008	27.821607
279.791153	10767.077635	27.826624
279.979156	10774.030122	27.831642
280.477203	10782.456004	27.836660
280.237339	10798.333378	27.841677
280.859929	10807.043593	27.846695
281.008043	10831.484882	27.851712
281.375023	10850.743270	27.856730
281.506901	10862.970455	27.861748
281.697845	10875.288577	27.866765
282.159181	10891.485165	27.871783
282.214635	10918.877216	27.876800
282.697992	10928.711083	27.881818
282.778355	10935.543078	27.886836
282.809594	10968.944983	27.891853
282.979170	10969.462132	27.896871
283.574386	10995.125453	27.901888
283.766857	11014.952528	27.906906
284.148422	11039.122816	27.911924
284.164030	11060.620202	27.916941
284.835417	11073.967642	27.921959
285.018365	11094.726176	27.926976
285.086231	11119.269652	27.931994
285.612993	11130.852134	27.937012
285.823347	11149.359494	27.942029
285.761607	11164.101160	27.947047
286.543075	11191.075393	27.952064
286.700282	11196.842644	27.957082
286.977705	11242.593337	27.962100
287.187820	11244.286117	27.967117
287.737494	11273.939023	27.972135
288.189184	11291.286216	27.977152
288.569681	11297.460217	27.982170
289.059839	11310.525886	27.987188
289.282078	11322.079923	27.992205
289.752905	11319.030751	27.997223
290.060775	11356.707350	28.002240
290.376174	11347.385681	28.007258
290.744833	11345.732809	28.012276
290.938225	11362.954800	28.017293
290.844024	11376.557927	28.022311
291.318301	11394.062584	28.027328
291.790787	11406.919841	28.032346
292.086529	11400.388086	28.037364
291.937013	11425.391693	28.042381
292.109955	11435.553971	28.047399
292.512171	11443.202388	28.052416
292.861442	11469.707293	28.057434
293.026755	11480.385132	28.062452
293.151532	11499.708926	28.067469
293.494257	11527.543069	28.072487
293.930177	11541.815428	28.077504
294.018221	11535.793651	28.082522
294.242478	11589.714876	28.087540
294.923628	11582.214970	28.092557
294.755651	11610.637108	28.097575
295.223586	11591.136017	28.102592
295.213586	11657.573068	28.107610
295.543783	11676.169799	28.112628
295.579670	11671.855079	28.117645
296.056007	11672.765280	28.122663
296.372019	11727.586506	28.127680
296.582605	11721.224411	28.132698
297.023776	11759.467108	28.137716
297.511966	11778.019896	28.142733
297.608203	11795.181523	28.147751
298.331971	11811.504132	28.152768
298.247109	11823.223193	28.157786
298.352235	11855.147070	28.162804
298.645850	11877.635479	28.167821
298.912651	11890.429519	28.172839
299.318600	11904.729036	28.177856
299.473031	11924.544089	28.182874
300.155208	11960.943024	28.187892
300.816767	11969.672897	28.192909
300.820160	11980.226571	28.197927
301.244185	11995.375267	28.202944
301.275191	12032.824181	28.207962
301.944160	12025.426349	28.212980
302.097986	12062.119874	28.217997
302.447216	12053.134748	28.223015
302.549182	12061.622513	28.228032
302.985390	12108.644432	28.233050
303.466816	12104.341617	28.238068
303.737804	12124.309932	28.243085
304.071942	12145.561336	28.248103
304.465289	12166.705345	28.253120
304.754868	12184.284827	28.258138
305.102073	12177.150314	28.263156
305.349324	12199.949215	28.268173
305.730429	12204.052755	28.273191
306.016333	12224.749607	28.278208
306.065928	12251.219825	28.283226
306.570857	12246.917947	28.288244
306.445790	12264.313321	28.293261
306.497585	12307.089556	28.298279
307.313322	12297.066971	28.303296
307.491264	12324.235841	28.308314
307.631739	12361.531567	28.313332
308.026658	12360.672291	28.318349
308.544271	12386.262008	28.323367
309.215607	12399.884148	28.328384
309.240919	12417.733480	28.333402
309.260051	12437.581787	28.338420
309.936121	12455.083659	28.343437
310.049297	12471.145197	28.348455
310.405817	12476.923285	28.353472
310.731378	12505.060660	28.358490
311.043579	12531.349024	28.363508
311.090925	12520.723859	28.368525
311.002065	12565.493278	28.373543
311.858341	12559.148355	28.378560
311.879626	12594.149261	28.383578
312.370603	12611.021833	28.388596
312.933813	12625.245814	28.393613
312.967029	12632.348385	28.398631
313.227272	12647.762128	28.403648
313.615155	12680.911061	28.408666
313.916285	12678.565952	28.413684
314.121959	12709.149772	28.418701
314.220226	12728.166496	28.423719
314.628983	12746.879142	28.428736
314.759339	12777.424926	28.433754
315.242507	12788.960740	28.438772
315.386074	12809.311934	28.443789
315.663404	12834.441888	28.448807
316.048216	12858.753499	28.453824
316.338147	12881.977163	28.458842
317.048706	12908.657636	28.463860
317.384692	12923.482848	28.468877
317.576359	12947.065050	28.473895
317.970900	12961.555112	28.478912
318.070623	12989.418476	28.483930
318.677418	13011.296676	28.488948
319.096711	13025.114806	28.493965
319.464398	13029.970818	28.498983
320.051017	13034.552466	28.504000
320.206420	13068.895150	28.509018
320.539562	13059.808495	28.514036
320.637899	13087.320032	28.519053
320.849796	13118.314159	28.524071
321.388603	13125.377120	28.529088
321.719218	13137.308633	28.534106
322.086721	13164.550927	28.539124
322.321499	13169.474604	28.544141
322.618499	13180.783399	28.549159
322.773830	13202.964643	28.554176
322.884140	13236.889855	28.559194
323.527418	13240.353110	28.564212
323.393271	13280.075272	28.569229
323.624320	13296.789322	28.574247
324.470460	13291.198984	28.579264
324.343244	13348.653446	28.584282
324.675587	13344.475979	28.589300
325.255638	13410.605697	28.594317
325.282995	13419.225754	28.599335
325.770968	13430.910258	28.604352
325.936398	13459.892347	28.609370
326.639730	13473.053243	28.614388
326.849150	13532.369815	28.619405
326.807068	13517.300333	28.624423
327.723153	13561.673447	28.629440
328.206712	13573.921756	28.634458
328.380207	13588.235908	28.639476
328.932492	13614.210822	28.644493
329.117361	13643.210629	28.649511
329.236013	13631.361934	28.654528
329.548251	13680.990271	28.659546
330.295585	13677.846597	28.664564
330.326514	13684.739271	28.669581
330.412900	13715.641270	28.674599
330.611806	13712.327594	28.679616
331.152470	13744.876357	28.684634
331.461116	13750.849707	28.689652
331.551428	13785.625303	28.694669
332.053432	13803.096068	28.699687
332.094312	13815.782122	28.704704
332.439291	13850.190422	28.709722
332.809420	13868.592213	28.714740
333.210732	13887.628609	28.719757
333.721746	13903.735119	28.724775
334.170926	13921.454715	28.729792
334.428241	13954.876566	28.734810
334.647629	13962.281971	28.739828
335.188334	14002.161672	28.744845
335.728764	14001.947316	28.749863
335.929711	14033.613538	28.754880
335.952551	14061.358778	28.759898
336.405375	14073.570573	28.764916
337.055157	14084.471476	28.769933
337.327867	14112.992973	28.774951
337.709296	14126.573142	28.779968
338.423694	14142.711158	28.784986
338.272804	14140.255736	28.790004
338.988487	14185.144447	28.795021
339.230636	14189.996735	28.800039
339.503804	14190.821411	28.805056
339.524285	14225.826887	28.810074
340.309589	14227.855974	28.815092
340.466148	14244.528329	28.820109
340.059629	14285.616580	28.825127
340.795432	14293.898519	28.830144
341.045998	14311.785416	28.835162
341.064195	14347.796669	28.840180
341.717420	14370.704757	28.845197
341.928132	14407.235677	28.850215
342.361940	14423.736525	28.855232
342.650633	14450.159677	28.860250
342.634266	14478.380879	28.865268
343.249602	14514.509880	28.870285
343.474137	14538.694944	28.875303
344.162558	14557.408457	28.880320
344.473920	14597.375659	28.885338
344.847450	14619.273774	28.890356
345.372109	14622.143933	28.895373
345.708464	14658.626307	28.900391
346.225259	14670.962113	28.905408
346.527802	14688.692983	28.910426
346.735748	14719.605490	28.915444
347.143693	14728.660484	28.920461
347.243338	14760.367285	28.925479
347.329501	14767.071970	28.930496
347.859184	14778.307585	28.935514
347.935364	14816.100643	28.940532
348.793756	14821.657474	28.945549
349.035350	14840.885924	28.950567
349.492869	14881.661657	28.955584
350.113295	14894.168581	28.960602
349.886394	14885.304112	28.965620
350.682748	14927.170060	28.970637
350.450168	14925.680526	28.975655
350.818545	14972.603057	28.980672
351.470713	14982.456962	28.985690
351.653562	15017.029327	28.990708
351.982157	15039.511339	28.995725
352.231896	15056.231232	29.000743
352.825592	15074.877624	29.005760
352.956192	15113.717597	29.010778
353.377957	15131.332370	29.015796
354.174852	15135.575531	29.020813
353.764968	15175.559767	29.025831
354.345767	15191.657115	29.030848
355.288640	15204.347207	29.035866
355.376270	15238.308233	29.040884
355.872470	15258.577479	29.045901
356.214925	15274.811691	29.050919
356.512314	15295.477539	29.055936
356.880555	15304.570102	29.060954
356.940096	15341.798051	29.065972
357.493575	15350.194746	29.070989
357.600643	15378.036112	29.076007
358.030617	15397.973262	29.081024
358.749778	15429.172292	29.086042
359.189674	15457.412337	29.091060
359.334482	15466.139805	29.096077
359.384408	15501.976389	29.101095
359.728024	15515.237127	29.106112
360.289239	15524.211296	29.111130
360.247049	15578.050662	29.116148
361.057226	15569.602006	29.121165
361.381298	15632.129898	29.126183
362.039550	15635.304882	29.131200
362.483163	15655.474200	29.136218
362.683149	15681.298493	29.141236
363.214807	15694.552548	29.146253
363.207199	15710.729839	29.151271
363.711946	15741.430026	29.156288
364.112386	15765.623247	29.161306
364.130872	15790.156052	29.166324
364.827189	15800.761174	29.171341
365.352222	15825.293224	29.176359
365.362561	15851.119386	29.181376
365.551949	15867.220677	29.186394
365.953793	15900.347726	29.191412
366.316135	15924.561046	29.196429
366.386905	15943.556835	29.201447
366.983064	15961.029150	29.206464
367.509676	15977.044644	29.211482
367.465123	16016.042935	29.216500
368.070323	16032.105598	29.221517
368.357442	16067.147483	29.226535
368.734185	16091.655861	29.231552
369.264203	16092.697252	29.236570
369.546910	16128.288499	29.241588
370.102615	16154.273008	29.246605
370.558896	16185.994223	29.251623
370.607614	16204.019810	29.256640
371.224391	16219.757262	29.261658
371.305165	16250.618923	29.266676
371.784039	16268.991917	29.271693
372.225077	16294.343277	29.276711
372.275233	16318.788920	29.281728
372.973357	16336.548910	29.286746
373.239873	16369.668718	29.291764
373.558992	16391.859689	29.296781
373.869671	16415.786691	29.301799
374.187975	16442.899003	29.306816
374.858070	16462.616141	29.311834
374.812621	16509.111363	29.316852
375.237364	16529.696487	29.321869
375.715636	16549.004411	29.326887
375.824688	16584.919811	29.331904
376.531717	16611.323139	29.336922
376.902653	16643.440041	29.341940
377.082776	16669.923687	29.346957
377.698249	16701.194384	29.351975
378.267635	16734.752277	29.356992
378.816036	16739.932021	29.362010
378.857877	16781.893746	29.367028
379.252360	16800.450878	29.372045
379.593134	16823.015051	29.377063
379.912333	16859.846886	29.382080
380.558298	16883.011839	29.387098
380.766741	16914.492492	29.392116
381.220264	16933.259442	29.397133
381.470812	16954.983967	29.402151
382.116179	16976.611169	29.407168
382.323405	17009.939020	29.412186
382.626887	17046.033346	29.417204
383.131715	17050.941041	29.422221
383.795933	17090.688754	29.427239
384.218429	17115.952802	29.432256
384.823320	17120.324953	29.437274
385.222588	17152.538981	29.442292
385.565008	17162.808972	29.447309
385.996177	17174.941187	29.452327
386.232040	17194.366885	29.457344
387.124784	17214.591974	29.462362
387.604819	17236.210260	29.467380
387.750009	17245.639586	29.472397
388.331079	17246.825375	29.477415
388.531244	17256.479190	29.482432
388.513477	17288.049990	29.487450
389.047296	17292.053636	29.492468
388.938223	17308.440483	29.497485
389.189504	17335.219217	29.502503
389.363144	17358.044246	29.507520
390.024451	17386.286515	29.512538
390.208611	17412.825514	29.517556
390.587927	17434.765608	29.522573
391.009746	17454.949329	29.527591
390.882356	17476.976714	29.532608
391.517701	17501.578998	29.537626
392.214118	17535.598668	29.542644
392.322630	17563.760461	29.547661
392.977713	17585.490507	29.552679
393.687980	17619.417612	29.557696
393.908306	17646.440381	29.562714
393.930446	17671.590799	29.567732
394.249699	17702.258620	29.572749
394.695460	17730.403198	29.577767
395.193605	17777.442935	29.582784
395.318732	17801.316819	29.587802
395.922561	17833.171748	29.592820
396.502425	17864.493985	29.597837
397.254317	17899.255171	29.602855
397.277478	17920.402959	29.607872
397.996964	17948.997989	29.612890
398.274815	17973.626494	29.617908
398.417701	18003.763207	29.622925
399.087282	18029.368494	29.627943
399.374874	18056.438738	29.632960
399.976414	18075.824801	29.637978
400.340863	18101.910493	29.642996
400.679736	18136.043177	29.648013
401.148525	18158.811732	29.653031
400.900645	18174.222843	29.658048
402.024071	18218.504590	29.663066
402.324589	18240.741836	29.668084
402.870395	18252.466892	29.673101
403.044836	18286.391472	29.678119
403.584969	18316.543843	29.683136
403.776952	18353.371950	29.688154
404.395293	18375.585916	29.693172
404.988189	18385.993779	29.698189
405.319469	18408.311400	29.703207
405.266250	18457.974428	29.708224
406.229322	18466.432878	29.713242
406.510965	18490.258477	29.718260
406.935007	18534.180923	29.723277
407.351895	18557.007152	29.728295
407.457032	18559.595422	29.733312
408.237444	18604.068358	29.738330
408.527811	18619.596508	29.743348
408.859700	18628.720561	29.748365
409.092619	18676.014732	29.753383
409.641985	18690.990281	29.758400
410.021087	18698.604912	29.763418
410.591337	18737.222844	29.768436
410.496330	18762.982073	29.773453
411.472013	18772.046157	29.778471
411.442684	18792.883225	29.783488
411.790376	18825.984539	29.788506
412.126175	18848.852858	29.793524
412.430429	18896.177278	29.798541
413.037926	18879.606535	29.803559
413.398416	18916.664642	29.808576
413.709843	18966.638518	29.813594
414.511321	18985.395051	29.818612
414.551814	18999.945283	29.823629
415.196979	19045.478831	29.828647
415.610255	19063.991403	29.833664
416.059654	19084.285656	29.838682
416.423670	19139.356470	29.843700
416.827465	19132.928262	29.848717
417.357441	19190.847651	29.853735
417.463378	19203.293129	29.858752
417.855653	19235.209849	29.863770
418.652205	19251.641468	29.868788
418.844949	19287.355507	29.873805
419.612342	19319.722488	29.878823
419.969082	19344.065005	29.883840
420.468363	19366.200149	29.888858
420.788961	19386.337362	29.893876
420.941915	19433.203650	29.898893
421.662958	19439.990131	29.903911
421.789421	19477.855389	29.908928
422.257512	19520.231824	29.913946
422.869140	19523.269894	29.918964
422.901319	19590.965703	29.923981
423.547242	19582.589212	29.928999
423.526455	19648.221972	29.934016
424.362003	19665.823067	29.939034
424.826300	19688.165041	29.944052
425.264518	19726.678116	29.949069
425.683931	19755.601672	29.954087
426.117024	19762.570007	29.959104
426.680136	19777.716871	29.964122
427.405547	19847.965297	29.969140
427.342918	19844.308901	29.974157
428.203096	19892.202934	29.979175
428.580483	19890.213140	29.984192
429.001731	19945.860006	29.989210
429.564901	19938.822973	29.994228
429.808604	19999.330505	29.999245
430.417488	19994.295746	30.004263
430.427309	20027.069956	30.009280
430.670171	20048.308673	30.014298
431.660975	20077.699707	30.019316
431.746244	20099.365992	30.024333
431.969976	20148.365432	30.029351
432.903433	20144.254580	30.034368
433.003575	20182.702950	30.039386
433.654193	20211.520041	30.044404
434.286327	20222.889904	30.049421
434.644933	20245.697978	30.054439
434.909438	20261.188581	30.059456
435.067663	20285.355125	30.064474
435.512253	20315.498254	30.069492
435.814545	20335.173036	30.074509
436.090440	20360.439551	30.079527
436.917219	20397.596202	30.084544
436.930373	20420.408382	30.089562
437.180394	20454.165787	30.094580
437.795371	20498.929978	30.099597
438.415003	20529.272821	30.104615
438.556649	20558.906360	30.109632
439.241840	20591.905686	30.114650
439.882090	20624.196025	30.119668
439.985812	20657.230246	30.124685
440.412860	20686.948101	30.129703
440.745419	20729.589992	30.134720
441.088646	20758.525971	30.139738
441.760867	20791.538811	30.144756
441.987054	20818.418109	30.149773
442.806261	20851.135185	30.154791
443.183106	20893.038095	30.159808
443.625662	20915.250630	30.164826
443.876918	20950.844964	30.169844
444.469012	20987.324571	30.174861
444.551969	21035.853089	30.179879
445.611500	21054.667097	30.184896
446.163552	21086.704298	30.189914
446.178824	21118.598307	30.194932
446.694368	21153.116996	30.199949
447.236651	21183.988073	30.204967
447.745065	21215.799386	30.209984
448.045228	21254.719773	30.215002
448.801944	21285.104066	30.220020
449.132892	21328.994092	30.225037
449.739877	21352.780508	30.230055
450.192002	21388.791935	30.235072
450.780328	21412.594803	30.240090
451.577924	21442.506281	30.245108
451.952214	21450.229746	30.250125
452.204966	21492.185921	30.255143
452.673003	21511.476665	30.260160
453.175352	21541.451119	30.265178
453.892967	21562.311879	30.270196
454.082200	21586.232930	30.275213
454.273365	21624.430137	30.280231
454.795858	21653.386464	30.285248
454.993636	21680.337525	30.290266
455.785527	21711.561677	30.295284
455.848285	21735.411749	30.300301
456.607456	21763.376863	30.305319
457.126216	21790.632160	30.310336
457.119439	21826.445208	30.315354
457.700940	21855.723277	30.320372
457.851386	21874.519294	30.325389
458.256643	21909.083994	30.330407
458.820823	21933.891689	30.335424
459.167646	21967.289226	30.340442
459.683502	22003.875489	30.345460
459.770291	22038.017887	30.350477
460.621612	22056.663090	30.355495
461.423375	22091.416256	30.360512
461.283501	22135.952158	30.365530
462.302085	22151.886823	30.370548
462.745026	22180.993045	30.375565
463.102368	22218.131938	30.380583
463.776659	22249.418426	30.385600
464.211402	22287.266563	30.390618
464.605405	22322.940499	30.395636
464.848413	22351.436229	30.400653
465.134502	22376.106996	30.405671
465.439597	22407.620366	30.410688
465.874938	22463.006539	30.415706
466.613983	22498.208491	30.420724
467.262817	22520.165982	30.425741
467.753659	22550.461590	30.430759
468.554946	22587.235290	30.435776
469.045700	22621.358703	30.440794
469.424140	22643.765835	30.445812
470.029323	22692.554144	30.450829
470.368786	22710.113674	30.455847
470.570730	22745.541144	30.460864
470.862840	22773.398955	30.465882
471.370316	22809.237850	30.470900
471.804007	22846.264461	30.475917
472.300896	22887.089915	30.480935
472.812041	22932.127652	30.485952
472.958307	22965.888472	30.490970
473.828543	23001.484929	30.495988
474.231359	23049.663107	30.501005
474.512990	23084.808494	30.506023
475.330080	23108.766521	30.511040
475.513160	23153.123885	30.516058
476.061485	23194.698835	30.521076
476.907437	23219.188009	30.526093
476.875666	23251.086736	30.531111
477.662963	23317.752066	30.536128
477.896886	23350.220648	30.541146
478.658045	23374.149396	30.546164
478.880916	23413.534405	30.551181
479.369303	23464.827085	30.556199
480.433651	23489.077107	30.561216
480.688967	23522.327900	30.566234
481.031331	23560.118980	30.571252
481.461902	23597.007649	30.576269
482.049783	23599.585627	30.581287
482.677007	23660.551807	30.586304
483.237034	23663.550892	30.591322
483.524397	23719.543167	30.596340
483.929822	23720.798641	30.601357
484.246456	23752.110432	30.606375
484.947496	23803.271091	30.611392
485.279598	23801.316790	30.616410
485.578030	23870.047183	30.621428
486.385676	23874.006389	30.626445
486.561308	23911.239646	30.631463
487.069102	23963.903723	30.636480
487.548630	23997.942106	30.641498
488.217257	24023.261822	30.646516
488.600384	24063.240440	30.651533
488.800833	24118.190144	30.656551
489.794659	24132.638951	30.661568
489.488112	24172.771026	30.666586
490.389153	24213.495354	30.671604
490.817402	24251.496524	30.676621
491.215444	24294.702778	30.681639
491.961906	24316.438492	30.686656
492.410281	24346.079517	30.691674
492.964924	24415.073133	30.696692
493.356749	24440.667610	30.701709
493.910520	24480.260128	30.706727
494.526637	24524.959577	30.711744
494.958246	24549.287606	30.716762
495.298049	24598.395814	30.721780
495.632892	24637.812499	30.726797
496.113905	24678.255984	30.731815
496.625882	24704.977046	30.736832
497.430922	24773.225773	30.741850
497.941482	24794.726393	30.746868
498.279814	24852.224546	30.751885
498.419080	24888.038578	30.756903
499.261783	24905.388841	30.761920
499.997091	24967.453478	30.766938
500.316739	25016.390528	30.771956
501.230849	25044.808623	30.776973
501.297626	25081.052907	30.781991
502.008504	25132.209193	30.787008
502.864761	25165.937217	30.792026
503.410243	25198.485197	30.797044
503.362760	25244.351844	30.802061
503.821740	25282.573505	30.807079
504.920295	25283.584794	30.812096
505.042669	25354.839614	30.817114
505.991876	25369.472330	30.822132
506.377302	25401.137977	30.827149
507.011887	25457.292169	30.832167
507.672694	25466.343405	30.837184
507.793259	25501.006986	30.842202
508.545737	25533.446270	30.847220
509.188749	25569.473052	30.852237
509.226421	25601.877451	30.857255
509.999956	25628.244098	30.862272
510.232040	25645.156777	30.867290
510.426858	25684.111534	30.872308
511.062963	25712.176513	30.877325
511.906632	25762.613374	30.882343
512.090691	25784.680159	30.887360
512.432954	25826.450010	30.892378
513.165455	25852.318621	30.897396
513.761313	25892.208078	30.902413
513.851363	25930.085942	30.907431
514.720706	25952.716542	30.912448
514.699043	26002.490065	30.917466
515.018172	26038.751466	30.922484
515.884623	26075.611907	30.927501
516.616878	26121.554597	30.932519
516.963883	26156.159896	30.937536
517.299367	26192.238644	30.942554
517.649450	26254.148286	30.947572
518.388121	26291.617251	30.952589
518.942045	26339.755330	30.957607
519.254504	26375.074809	30.962624
519.753173	26431.941798	30.967642
520.167708	26474.896094	30.972660
521.069246	26525.041757	30.977677
521.402818	26559.117529	30.982695
521.900555	26608.803899	30.987712
522.689482	26666.066645	30.992730
523.445703	26683.136425	30.997748
523.784359	26737.798978	31.002765
524.471813	26766.856549	31.007783
524.967454	26804.983054	31.012800
525.962038	26850.682804	31.017818
526.116324	26893.302319	31.022836
526.745107	26926.436127	31.027853
526.967286	26954.716538	31.032871
527.981714	27002.342881	31.037888
528.290155	27036.408701	31.042906
528.821571	27073.226332	31.047924
529.457732	27122.253335	31.052941
529.878672	27164.159885	31.057959
530.163359	27197.336454	31.062976
531.108801	27236.404679	31.067994
531.735067	27280.768317	31.073012
532.129132	27308.075807	31.078029
532.695117	27336.806334	31.083047
533.265565	27379.682283	31.088064
533.305528	27418.470536	31.093082
533.881724	27473.545240	31.098100
534.988647	27504.075171	31.103117
535.189600	27546.095749	31.108135
535.510681	27575.793771	31.113152
536.065826	27614.824240	31.118170
536.397320	27676.705296	31.123188
537.393806	27702.448196	31.128205
537.908321	27741.568954	31.133223
538.121452	27787.278451	31.138240
538.760652	27824.398136	31.143258
538.847114	27861.598063	31.148276
539.898820	27882.402137	31.153293
540.265150	27919.800279	31.158311
540.740616	27970.146742	31.163328
541.294642	27983.855281	31.168346
541.147478	28055.317852	31.173364
542.445089	28072.478583	31.178381
542.940379	28118.626245	31.183399
543.350510	28169.604567	31.188416
544.044081	28211.693385	31.193434
544.406540	28248.827398	31.198452
545.055088	28287.819410	31.203469
545.246947	28335.037091	31.208487
545.892793	28397.804466	31.213504
546.891832	28414.874455	31.218522
547.311835	28466.903162	31.223540
547.884481	28507.781355	31.228557
548.082107	28552.419251	31.233575
548.682534	28594.252873	31.238592
549.505623	28646.750565	31.243610
549.856422	28697.886549	31.248628
550.701342	28738.224019	31.253645
551.173653	28767.588934	31.258663
551.669725	28834.743604	31.263680
552.470447	28838.763504	31.268698
553.078100	28922.563088	31.273716
553.551688	28930.330340	31.278733
554.253462	28994.512487	31.283751
554.946213	29029.329694	31.288768
555.301137	29042.265614	31.293786
555.699886	29095.796739	31.298804
556.297387	29131.053227	31.303821
556.905826	29174.336820	31.308839
557.193278	29228.020051	31.313856
557.987409	29258.067359	31.318874
558.312128	29302.023656	31.323892
559.177890	29348.995139	31.328909
559.819839	29390.723356	31.333927
560.371874	29421.105781	31.338944
561.182455	29460.695699	31.343962
561.481149	29513.349059	31.348980
562.393540	29553.660486	31.353997
562.618532	29594.998638	31.359015
563.024354	29629.241947	31.364032
563.707691	29659.947446	31.369050
564.134364	29710.570265	31.374068
564.668151	29744.030717	31.379085
565.446294	29806.984196	31.384103
565.595198	29828.324608	31.389120
566.648329	29901.425860	31.394138
566.865100	29922.025952	31.399156
567.341519	29977.238540	31.404173
567.990734	30014.173342	31.409191
568.184598	30053.494167	31.414208
569.296706	30095.078403	31.419226
569.629275	30127.188048	31.424244
569.869636	30178.470782	31.429261
570.474255	30212.886953	31.434279
570.831817	30244.031541	31.439296
571.870514	30283.721092	31.444314
572.096443	30340.889551	31.449332
572.971045	30393.064786	31.454349
573.529603	30437.021582	31.459367
573.718684	30476.224418	31.464384
574.216206	30517.956470	31.469402
574.715189	30573.466915	31.474420
575.029780	30621.768557	31.479437
575.998943	30666.004137	31.484455
576.828042	30720.743873	31.489472
577.176213	30771.067298	31.494490
577.716948	30821.147454	31.499508
578.565411	30867.476786	31.504525
579.316719	30907.260909	31.509543
579.641104	30950.583439	31.514560
580.239358	31008.246534	31.519578
580.974661	31066.146471	31.524596
581.451566	31102.258570	31.529613
582.048276	31157.353557	31.534631
582.639140	31209.010806	31.539648
583.282655	31258.393523	31.544666
583.612400	31298.532572	31.549684
584.386040	31362.342253	31.554701
585.201345	31401.165471	31.559719
585.553877	31447.378424	31.564736
586.430821	31483.850037	31.569754
586.709184	31532.965496	31.574772
587.446594	31587.732198	31.579789
588.083149	31631.708160	31.584807
588.548750	31680.069258	31.589824
589.540114	31731.421664	31.594842
589.468706	31792.607916	31.599860
590.418400	31819.768328	31.604877
591.102992	31866.024146	31.609895
591.402912	31930.470989	31.614912
592.189498	31972.282081	31.619930
592.797816	32018.481128	31.624948
593.299812	32068.315947	31.629965
594.071206	32129.471683	31.634983
594.885951	32165.549667	31.640000
595.465708	32210.756132	31.645018
595.860663	32259.171167	31.650036
596.207382	32303.169869	31.655053
596.957250	32355.141125	31.660071
597.299630	32414.329895	31.665088
598.174176	32464.402900	31.670106
598.849551	32508.696564	31.675124
599.432043	32560.860619	31.680141
599.919210	32601.218937	31.685159
600.420406	32644.929162	31.690176
601.246305	32675.240942	31.695194
601.568070	32718.934230	31.700212
602.027515	32755.787244	31.705229
602.667696	32807.917678	31.710247
603.100494	32861.777260	31.715264
604.048823	32903.464095	31.720282
604.709687	32957.490998	31.725300
604.750640	32999.754445	31.730317
605.815689	33043.008687	31.735335
606.352263	33100.819786	31.740352
607.040622	33136.582728	31.745370
607.583020	33195.420911	31.750388
607.943963	33232.683152	31.755405
608.823975	33279.509215	31.760423
609.254658	33331.685702	31.765440
609.835375	33376.772275	31.770458
610.385728	33440.802129	31.775476
611.388556	33477.513485	31.780493
612.049705	33534.858619	31.785511
612.597632	33568.129194	31.790528
613.408889	33623.210901	31.795546
613.811154	33680.326652	31.800564
614.346954	33723.370628	31.805581
615.008013	33772.264746	31.810599
615.571213	33821.787757	31.815616
615.827631	33856.274917	31.820634
616.670804	33927.012742	31.825652
617.298759	33978.097451	31.830669
618.074905	34035.976134	31.835687
618.190783	34091.463322	31.840704
619.214841	34128.093934	31.845722
619.844310	34185.517304	31.850740
620.025688	34266.041992	31.855757
621.020980	34301.983998	31.860775
621.627452	34368.426561	31.865792
622.070629	34418.969854	31.870810
622.619418	34480.533892	31.875828
623.495421	34531.133134	31.880845
623.982053	34584.753310	31.885863
624.301751	34656.282228	31.890880
625.207195	34695.515031	31.895898
625.991353	34759.790194	31.900916
626.320778	34823.974075	31.905933
627.098918	34870.305402	31.910951
628.046559	34931.772924	31.915968
628.623237	34988.037816	31.920986
629.689859	35037.832678	31.926004
630.118962	35087.595213	31.931021
630.860594	35138.826190	31.936039
631.155478	35190.147379	31.941056
632.049129	35236.248523	31.946074
633.006367	35288.155007	31.951092
633.108508	35346.024204	31.956109
634.211755	35372.379420	31.961127
634.727190	35426.727604	31.966144
635.053928	35456.871759	31.971162
635.554497	35516.520936	31.976180
636.265800	35552.223972	31.981197
636.813163	35601.280314	31.986215
636.922870	35652.615074	31.991232
638.018808	35701.171335	31.996250
638.471247	35762.386577	32.001268
638.879277	35804.746901	32.006285
639.891462	35864.547596	32.011303
640.175960	35909.488017	32.016320
640.810708	35970.156338	32.021338
641.271587	36019.829892	32.026356
641.963534	36086.141167	32.031373
642.545639	36146.593076	32.036391
642.820618	36210.888709	32.041408
643.712929	36270.225966	32.046426
644.818184	36325.679720	32.051444
645.035405	36397.500432	32.056461
646.297274	36444.588363	32.061479
646.785611	36508.073948	32.066496
647.581274	36555.129222	32.071514
648.207977	36615.738107	32.076532
648.832492	36682.130275	32.081549
649.698164	36735.127891	32.086567
650.294624	36791.116672	32.091584
650.999353	36846.755749	32.096602
651.629787	36899.278964	32.101620
652.261385	36954.964730	32.106637
652.983399	36994.277887	32.111655
653.504516	37069.677604	32.116672
653.959883	37114.240903	32.121690
654.790219	37174.062632	32.126708
654.982694	37241.561618	32.131725
655.896778	37300.046132	32.136743
656.274970	37366.781361	32.141760
656.950620	37420.993850	32.146778
657.987729	37481.412816	32.151796
658.410586	37543.257309	32.156813
659.075548	37603.833720	32.161831
659.920767	37670.699178	32.166848
660.198756	37730.500473	32.171866
661.348760	37797.150783	32.176884
661.754541	37856.575859	32.181901
662.759853	37920.924153	32.186919
663.290698	37991.498764	32.191936
663.874236	38046.243502	32.196954
665.048219	38096.309471	32.201972
665.652743	38162.351196	32.206989
666.278114	38206.660130	32.212007
666.717122	38266.234298	32.217024
667.312298	38318.143199	32.222042
668.138411	38380.809506	32.227060
669.016978	38431.710279	32.232077
669.706646	38475.867782	32.237095
670.126317	38546.296863	32.242112
670.707058	38583.173422	32.247130
671.498951	38627.559437	32.252148
672.019371	38679.522348	32.257165
672.806507	38728.666345	32.262183
673.347159	38777.064519	32.267200
673.694818	38835.988287	32.272218
674.684639	38878.408799	32.277236
675.118499	38942.137720	32.282253
676.034351	38995.708415	32.287271
676.403766	39054.918027	32.292288
676.716524	39116.263913	32.297306
677.918401	39156.256266	32.302324
678.115344	39234.285827	32.307341
678.986633	39293.859441	32.312359
680.098639	39353.103236	32.317376
680.372885	39419.883633	32.322394
681.010546	39471.537029	32.327412
681.559953	39548.581612	32.332429
682.665990	39604.594801	32.337447
682.983963	39664.221548	32.342464
683.467861	39735.895762	32.347482
684.377735	39797.388721	32.352500
684.748549	39866.828214	32.357517
685.350803	39953.697748	32.362535
686.544789	40011.927929	32.367552
687.433515	40074.719847	32.372570
688.187378	40133.802636	32.377588
688.547702	40203.150562	32.382605
689.392417	40256.318706	32.387623
689.932114	40322.281416	32.392640
690.756468	40402.621179	32.397658
691.770519	40457.782975	32.402676
692.556766	40529.396629	32.407693
693.029874	40575.620394	32.412711
693.646240	40633.785405	32.417728
694.736551	40706.404765	32.422746
695.411706	40762.922453	32.427764
696.002309	40824.436847	32.432781
696.789875	40881.782260	32.437799
697.191165	40932.194116	32.442816
697.493396	41000.960036	32.447834
698.805896	41063.252906	32.452852
699.580324	41128.219434	32.457869
700.070529	41195.366650	32.462887
700.980761	41270.048195	32.467904
701.945134	41332.887908	32.472922
702.442525	41389.163159	32.477940
702.856008	41438.368187	32.482957
703.221373	41495.226208	32.487975
704.248860	41548.654725	32.492992
704.715854	41630.069588	32.498010
705.839804	41687.577052	32.503028
706.603502	41760.249744	32.508045
706.704965	41819.270347	32.513063
707.281737	41871.043225	32.518080
708.047600	41942.912071	32.523098
708.879055	41997.906065	32.528116
709.628408	42071.411876	32.533133
710.256048	42121.243973	32.538151
711.014808	42181.741371	32.543168
711.635607	42248.105485	32.548186
712.475439	42303.988583	32.553204
712.846717	42372.865722	32.558221
713.786718	42428.446255	32.563239
714.343914	42495.155787	32.568256
715.087778	42561.022089	32.573274
715.903966	42626.905518	32.578292
716.648811	42691.299169	32.583309
716.819578	42769.700739	32.588327
717.687153	42832.857864	32.593344
718.449356	42910.374214	32.598362
719.289581	42980.510211	32.603380
720.015923	43052.036719	32.608397
720.552044	43121.168185	32.613415
721.283921	43191.710264	32.618432
722.006641	43273.669438	32.623450
723.211693	43335.374182	32.628468
723.725428	43418.742588	32.633485
724.567864	43476.963277	32.638503
725.328909	43561.226680	32.643520
725.797430	43628.143978	32.648538
726.730029	43701.249064	32.653556
727.447703	43771.199601	32.658573
728.127348	43847.055181	32.663591
728.923542	43929.819606	32.668608
729.579847	44004.105543	32.673626
730.560057	44060.536643	32.678644
731.068853	44137.890659	32.683661
732.014060	44205.500837	32.688679
733.101843	44263.997417	32.693696
733.398583	44341.231530	32.698714
734.443218	44410.933875	32.703732
735.129665	44481.469530	32.708749
735.938927	44550.664178	32.713767
736.594160	44603.234030	32.718784
737.144220	44687.075943	32.723802
738.391574	44747.722237	32.728820
738.590579	44825.270591	32.733837
739.262847	44892.693465	32.738855
740.445220	44961.921843	32.743872
740.900099	45032.357799	32.748890
741.613900	45094.759028	32.753908
742.573357	45167.998529	32.758925
742.929050	45250.785758	32.763943
744.021565	45312.111687	32.768960
744.788020	45387.136823	32.773978
745.543765	45442.677534	32.778996
746.246672	45526.552796	32.784013
746.874445	45598.641819	32.789031
747.576137	45646.188298	32.794048
748.226648	45719.555016	32.799066
748.379671	45780.584180	32.804084
749.311480	45852.685796	32.809101
750.181312	45931.252226	32.814119
751.011063	45988.032185	32.819136
751.784098	46060.544818	32.824154
752.597797	46114.564149	32.829172
753.287917	46193.242392	32.834189
753.855050	46264.886375	32.839207
754.725135	46327.106248	32.844224
755.213740	46414.275685	32.849242
755.737308	46487.889834	32.854260
756.592816	46568.521541	32.859277
757.112454	46648.099716	32.864295
758.011356	46723.355599	32.869312
758.210313	46810.888607	32.874330
759.301028	46896.090574	32.879348
760.296054	46977.241450	32.884365
761.000543	47066.244345	32.889383
761.996444	47144.859263	32.894400
762.470625	47234.221479	32.899418
763.591493	47303.358528	32.904436
764.690797	47380.547753	32.909453
765.359877	47456.720467	32.914471
766.405774	47542.172493	32.919488
767.052590	47621.296287	32.924506
767.772552	47678.294824	32.929524
768.606435	47761.024123	32.934541
769.186925	47848.268091	32.939559
770.239708	47903.627362	32.944576
770.694982	48009.368453	32.949594
771.386136	48080.482669	32.954612
772.318818	48165.081766	32.959629
773.060942	48235.361840	32.964647
773.726113	48301.514832	32.969664
774.462207	48392.030744	32.974682
775.683757	48470.173947	32.979700
776.416987	48549.032582	32.984717
777.004611	48648.935031	32.989735
778.122558	48706.684451	32.994752
778.998779	48789.440238	32.999770
779.938644	48855.854491	33.004788
780.455525	48926.217344	33.009805
781.551544	49006.149874	33.014823
782.059486	49083.907686	33.019840
782.921913	49169.125450	33.024858
783.504745	49234.449410	33.029876
784.300243	49308.975530	33.034893
784.862973	49386.287353	33.039911
785.929833	49466.106699	33.044928
786.604820	49531.047903	33.049946
787.290184	49617.233163	33.054964
787.841686	49695.561013	33.059981
788.903638	49771.769539	33.064999
789.462331	49836.749306	33.070016
790.124015	49916.947564	33.075034
791.086038	49993.043572	33.080052
791.703193	50063.101516	33.085069
792.439515	50137.425963	33.090087
793.332765	50199.466508	33.095104
793.860354	50288.195093	33.100122
794.500812	50366.092053	33.105140
795.480425	50443.929061	33.110157
795.848777	50532.438072	33.115175
796.884669	50611.273488	33.120192
797.664606	50698.420862	33.125210
798.149030	50770.026878	33.130228
799.354701	50865.195188	33.135245
799.565697	50960.490765	33.140263
800.553002	51050.147161	33.145280
801.776060	51128.866718	33.150298
802.314011	51213.044589	33.155316
803.253628	51305.985487	33.160333
804.318049	51395.909051	33.165351
805.097075	51463.564152	33.170368
805.906454	51571.494898	33.175386
806.633903	51653.236828	33.180404
807.810186	51727.750341	33.185421
808.633789	51824.016518	33.190439
809.348342	51904.373087	33.195456
810.310758	51993.662635	33.200474
810.877396	52084.959628	33.205492
811.831214	52165.112025	33.210509
812.637961	52246.294917	33.215527
813.417208	52332.181694	33.220544
814.200894	52415.047961	33.225562
815.003722	52505.889766	33.230580
816.059529	52573.284092	33.235597
816.908515	52663.219902	33.240615
817.466857	52749.882329	33.245632
818.559114	52848.348829	33.250650
819.197080	52909.274852	33.255668
820.054508	53000.009471	33.260685
820.592919	53104.571430	33.265703
821.601999	53183.681238	33.270720
822.359097	53269.942120	33.275738
823.049264	53365.189972	33.280756
824.526468	53427.678999	33.285773
824.870451	53521.215356	33.290791
825.893223	53610.446516	33.295808
826.569713	53705.496347	33.300826
827.593389	53777.356774	33.305844
828.407659	53853.464301	33.310861
829.094448	53972.371407	33.315879
830.203893	54036.328737	33.320896
831.286331	54107.941256	33.325914
832.044165	54207.970758	33.330932
833.197249	54263.775715	33.335949
833.767733	54355.579121	33.340967
834.105222	54429.419850	33.345984
835.233774	54500.237515	33.351002
835.811401	54573.838613	33.356020
836.616077	54652.242496	33.361037
837.185373	54727.382665	33.366055
838.000599	54803.374092	33.371072
838.862261	54892.829751	33.376090
839.450803	54980.735350	33.381108
840.546681	55055.527938	33.386125
840.952627	55158.797156	33.391143
841.693030	55234.795982	33.396160
842.401136	55319.060628	33.401178
843.266767	55427.204330	33.406196
844.368790	55514.926628	33.411213
845.186457	55619.957369	33.416231
845.885681	55714.013494	33.421248
846.895653	55803.803553	33.426266
847.665766	55896.476256	33.431284
848.553007	55986.728661	33.436301
849.388469	56087.646289	33.441319
850.417237	56181.668161	33.446336
851.508056	56272.290465	33.451354
852.070536	56362.182893	33.456372
853.057469	56459.839794	33.461389
853.835099	56553.512123	33.466407
854.814177	56652.613886	33.471424
855.766469	56744.235979	33.476442
856.471021	56843.259350	33.481460
857.662301	56936.460597	33.486477
858.611966	57023.469403	33.491495
859.561773	57122.600462	33.496512
860.423629	57205.836024	33.501530
860.845873	57303.015908	33.506548
861.543070	57399.669561	33.511565
862.598427	57496.711835	33.516583
863.221512	57586.089211	33.521600
864.152411	57687.420312	33.526618
864.740965	57799.542899	33.531636
865.836170	57881.866782	33.536653
866.482458	57994.675879	33.541671
867.367949	58099.504830	33.546688
868.532149	58199.381013	33.551706
869.251466	58313.136981	33.556724
870.250338	58391.071381	33.561741
871.181053	58498.313626	33.566759
872.318883	58588.883050	33.571776
873.791528	58678.900833	33.576794
874.591791	58778.557090	33.581812
875.436426	58862.159616	33.586829
876.463867	58965.929074	33.591847
877.311085	59047.486257	33.596864
877.856034	59133.925387	33.601882
878.940026	59222.321782	33.606900
879.964915	59305.345134	33.611917
880.837668	59396.336389	33.616935
881.349390	59471.495664	33.621952
882.446148	59538.748204	33.626970
883.098586	59637.447571	33.631988
883.993924	59728.162185	33.637005
884.722366	59801.113010	33.642023
885.205683	59889.743928	33.647040
886.318895	59960.477779	33.652058
886.877586	60055.752913	33.657076
887.523674	60169.045702	33.662093
888.388659	60254.012035	33.667111
889.497026	60358.641487	33.672128
890.354589	60445.627382	33.677146
890.709822	60558.814111	33.682164
891.649625	60648.831523	33.687181
892.796266	60754.088571	33.692199
893.341709	60871.335699	33.697216
894.372911	60972.106772	33.702234
895.200626	61086.490783	33.707252
896.068038	61166.014349	33.712269
897.012742	61300.462273	33.717287
897.706213	61411.105952	33.722304
899.098695	61500.963869	33.727322
899.795653	61611.892351	33.732340
901.136702	61723.606263	33.737357
901.982225	61830.196070	33.742375
902.855160	61941.505820	33.747392
903.793463	62035.789679	33.752410
904.596114	62155.571010	33.757428
905.763760	62257.555584	33.762445
906.614757	62368.233514	33.767463
907.508517	62467.774599	33.772480
908.936770	62563.416714	33.777498
909.350197	62684.103274	33.782516
910.096394	62777.253074	33.787533
911.548627	62876.072758	33.792551
911.968740	62995.895035	33.797568
913.066033	63096.670147	33.802586
914.034011	63211.480532	33.807604
915.006648	63309.993552	33.812621
915.867056	63429.331689	33.817639
916.784990	63536.134350	33.822656
918.087325	63626.626224	33.827674
918.613293	63742.735402	33.832692
919.685210	63845.669041	33.837709
920.710076	63944.669681	33.842727
921.151756	64053.452083	33.847744
922.123486	64157.129671	33.852762
923.311625	64267.174539	33.857780
923.931022	64382.369589	33.862797
924.882500	64489.014378	33.867815
925.804135	64602.034192	33.872832
927.289347	64701.742400	33.877850
927.529573	64816.690922	33.882868
928.713915	64927.021277	33.887885
929.895929	65026.094129	33.892903
930.472676	65130.108299	33.897920
931.550596	65219.790790	33.902938
932.293475	65322.497387	33.907956
933.223987	65417.222506	33.912973
933.934203	65520.096427	33.917991
934.759941	65623.100954	33.923008
935.786993	65722.069431	33.928026
936.736047	65843.016111	33.933044
937.613441	65946.731074	33.938061
938.778839	66043.357910	33.943079
939.642306	66158.944887	33.948096
940.314042	66271.455325	33.953114
941.298614	66368.248375	33.958132
942.349840	66476.934960	33.963149
943.198284	66596.203228	33.968167
943.924244	66720.958819	33.973184
945.291109	66815.893045	33.978202
946.072965	66929.378380	33.983220
946.662270	67047.796854	33.988237
948.006938	67154.204434	33.993255
948.669947	67269.526770	33.998272
949.312328	67407.473943	34.003290
950.888097	67522.769436	34.008308
951.861347	67637.466610	34.013325
953.019900	67745.909553	34.018343
953.525508	67869.062040	34.023360
954.893740	67983.063560	34.028378
955.769506	68099.936278	34.033396
956.373959	68225.090471	34.038413
957.808984	68327.383973	34.043431
959.255518	68449.278621	34.048448
960.145601	68547.591672	34.053466
961.086608	68666.226266	34.058484
962.053119	68771.521573	34.063501
963.228576	68880.410395	34.068519
963.691951	68999.148279	34.073536
965.389338	69108.125912	34.078554
966.266317	69212.174357	34.083572
966.780535	69319.907337	34.088589
968.246420	69425.600556	34.093607
969.060314	69538.897076	34.098624
970.202451	69643.467907	34.103642
971.137093	69751.509126	34.108660
972.189069	69865.628871	34.113677
973.500925	69961.721308	34.118695
973.864078	70072.590805	34.123712
974.798689	70162.830804	34.128730
975.667611	70272.407951	34.133748
976.494328	70399.669867	34.138765
977.688639	70495.012843	34.143783
978.581059	70606.654082	34.148800
979.466661	70706.425542	34.153818
980.135753	70841.189577	34.158836
981.798985	70941.798865	34.163853
982.229681	71055.259894	34.168871
983.255214	71165.170928	34.173888
984.333343	71265.742278	34.178906
985.574064	71363.691497	34.183924
985.712583	71482.413982	34.188941
987.079937	71583.490632	34.193959
987.917289	71684.273017	34.198976
988.692405	71797.917310	34.203994
989.602385	71903.440650	34.209012
990.574393	72030.993291	34.214029
991.865970	72137.752454	34.219047
992.372329	72250.784989	34.224064
993.212033	72372.743754	34.229082
994.253089	72500.004103	34.234100
995.150721	72616.281087	34.239117
996.102111	72737.504012	34.244135
997.121558	72874.096510	34.249152
998.192195	72995.466328	34.254170
999.181460	73128.451072	34.259188
999.794980	73264.289390	34.264205
1001.366997	73386.883516	34.269223
1001.970393	73522.036451	34.274240
1003.305597	73641.251301	34.279258
1004.339891	73765.317144	34.284276
1005.110870	73905.760271	34.289293
1006.294320	74042.675932	34.294311
1007.861808	74153.130291	34.299328
1008.553199	74279.667772	34.304346
1009.970352	74402.570829	34.309364
1010.741184	74528.484289	34.314381
1011.950861	74658.455199	34.319399
1013.024909	74770.539682	34.324416
1013.781733	74918.941834	34.329434
1015.480395	75024.577460	34.334452
1016.191189	75148.324188	34.339469
1017.025023	75273.884743	34.344487
1018.421662	75397.163699	34.349504
1019.476151	75508.730905	34.354522
1020.466473	75623.108497	34.359540
1021.284665	75750.197527	34.364557
1022.442390	75865.851706	34.369575
1023.360633	75996.282094	34.374592
1024.769525	76111.600708	34.379610
1026.020543	76228.525030	34.384628
1026.870518	76341.462847	34.389645
1027.688263	76471.766943	34.394663
1029.015710	76594.527056	34.399680
1029.817695	76699.972850	34.404698
1031.021483	76805.829274	34.409716
1031.662250	76940.771763	34.414733
1033.279407	77059.791443	34.419751
1033.986311	77187.747782	34.424768
1035.079211	77296.259865	34.429786
1035.919153	77411.537357	34.434804
1036.946480	77537.953391	34.439821
1038.145128	77652.941352	34.444839
1039.154934	77762.107483	34.449856
1039.757999	77875.851554	34.454874
1040.925300	77985.910270	34.459892
1041.543784	78096.676269	34.464909
1043.276407	78202.057685	34.469927
1043.940488	78322.152817	34.474944
1044.745030	78438.693197	34.479962
1045.984300	78545.956186	34.484980
1046.503162	78687.951682	34.489997
1047.453877	78788.606357	34.495015
1048.387396	78929.526290	34.500032
1049.698796	79051.020721	34.505050
1050.854892	79178.203880	34.510068
1051.716730	79301.838160	34.515085
1052.815772	79456.849500	34.520103
1053.877332	79552.610692	34.525120
1054.980150	79705.019151	34.530138
1056.299551	79825.613026	34.535156
1056.915001	79955.301561	34.540173
1058.030804	80084.993501	34.545191
1059.324758	80217.647743	34.550208
1060.401757	80351.222289	34.555226
1061.471260	80486.290661	34.560244
1062.340446	80622.371548	34.565261
1063.487912	80748.617633	34.570279
1064.762889	80889.123743	34.575296
1065.767950	81024.344951	34.580314
1067.063796	81148.085638	34.585332
1068.361703	81280.455306	34.590349
1068.988048	81409.790928	34.595367
1070.095732	81547.635229	34.600384
1071.478822	81691.144886	34.605402
1072.569016	81795.016001	34.610420
1073.650721	81954.985915	34.615437
1074.877235	82051.156008	34.620455
1075.966473	82202.213270	34.625472
1077.151645	82335.125966	34.630490
1078.135862	82445.901431	34.635508
1078.976710	82599.795252	34.640525
1079.983230	82724.963162	34.645543
1081.324754	82835.917776	34.650560
1082.080373	82996.105590	34.655578
1083.339639	83105.146564	34.660596
1083.932727	83247.332243	34.665613
1085.267929	83385.222061	34.670631
1086.536374	83531.658073	34.675648
1087.351315	83658.208619	34.680666
1088.648624	83804.787355	34.685684
1089.885891	83934.913910	34.690701
1090.841045	84099.149851	34.695719
1092.324428	84191.103684	34.700736
1093.176178	84348.397301	34.705754
1094.509405	84470.293021	34.710772
1094.966727	84607.698258	34.715789
1096.220623	84760.897369	34.720807
1097.768525	84865.735162	34.725824
1098.671382	84998.766550	34.730842
1099.323669	85102.021933	34.735860
1100.593490	85237.955372	34.740877
1101.501913	85344.060581	34.745895
1102.811673	85504.122457	34.750912
1103.826182	85625.525473	34.755930
1104.730449	85740.434397	34.760948
1105.798302	85878.616994	34.765965
1106.814426	86008.728280	34.770983
1108.149326	86156.727339	34.776000
1108.833376	86272.464510	34.781018
1110.471977	86434.049158	34.786036
1111.421723	86558.566002	34.791053
1112.176679	86699.067283	34.796071
1113.459182	86836.994345	34.801088
1114.482900	86985.345832	34.806106
1115.659324	87110.481120	34.811124
1116.562146	87274.041798	34.816141
1117.584688	87414.334506	34.821159
1119.231169	87552.429616	34.826176
1119.968368	87706.326508	34.831194
1121.087514	87849.768317	34.836212
1122.075206	88017.602024	34.841229
1123.175294	88148.566644	34.846247
1124.672492	88302.953995	34.851264
1125.547717	88457.169456	34.856282
1127.117004	88617.883695	34.861300
1128.482508	88751.364468	34.866317
1129.924817	88884.625177	34.871335
1131.180303	89031.037907	34.876352
1132.212679	89180.098778	34.881370
1133.672318	89292.111783	34.886388
1134.851655	89439.064255	34.891405
1135.773570	89588.752588	34.896423
1136.792361	89712.745545	34.901440
1138.092648	89845.750196	34.906458
1139.197929	90002.431699	34.911476
1140.475467	90138.439289	34.916493
1141.244783	90270.449586	34.921511
1142.704626	90400.232335	34.926528
1143.743593	90561.083286	34.931546
1144.759732	90673.755771	34.936564
1145.869097	90835.463954	34.941581
1147.038538	90967.326311	34.946599
1148.283093	91120.692500	34.951616
1149.611315	91256.041295	34.956634
1150.648429	91382.108885	34.961652
1151.870106	91558.457954	34.966669
1152.873156	91665.736652	34.971687
1154.010705	91818.840156	34.976704
1155.280766	91962.708917	34.981722
1156.193931	92101.189977	34.986740
1157.665860	92250.005905	34.991757
1158.282392	92398.674253	34.996775
1159.798839	92508.500140	35.001792
1160.280378	92665.862809	35.006810
1161.893968	92784.858041	35.011828
1162.862722	92917.042325	35.016845
1163.334140	93060.722699	35.021863
1164.934619	93199.025477	35.026880
1165.817939	93344.533319	35.031898
1167.072204	93469.895268	35.036916
1168.463740	93618.998870	35.041933
1169.633242	93773.350563	35.046951
1170.828428	93906.105629	35.051968
1172.019364	94048.406675	35.056986
1172.829008	94185.753459	35.062004
1174.066163	94337.150823	35.067021
1174.913950	94519.300935	35.072039
1176.333901	94635.376724	35.077056
1177.306001	94800.368018	35.082074
1178.170040	94981.412400	35.087092
1179.431115	95112.102133	35.092109
1180.496679	95286.918097	35.097127
1182.267548	95459.694019	35.102144
1183.158832	95600.136007	35.107162
1184.543403	95780.471543	35.112180
1186.053090	95923.284193	35.117197
1187.100358	96086.362693	35.122215
1188.622904	96241.877205	35.127232
1189.462845	96411.980907	35.132250
1190.707731	96562.436924	35.137268
1191.738451	96713.573231	35.142285
1192.454419	96876.260998	35.147303
1194.285321	97056.611714	35.152320
1195.130964	97228.030127	35.157338
1196.419186	97376.574247	35.162356
1197.841298	97557.126801	35.167373
1198.760954	97738.817141	35.172391
1200.408840	97884.498623	35.177408
1201.647631	98054.253941	35.182426
1202.565734	98223.511133	35.187444
1204.335185	98392.134451	35.192461
1205.666106	98542.267313	35.197479
1206.719860	98699.499127	35.202496
1207.665715	98863.853736	35.207514
1208.892902	99035.237776	35.212532
1210.416700	99160.228025	35.217549
1211.387607	99368.260414	35.222567
1212.880786	99498.894340	35.227584
1214.091893	99692.871782	35.232602
1215.480826	99840.574527	35.237620
1216.845817	99976.982513	35.242637
1217.708835	100166.837344	35.247655
1219.134071	100289.888133	35.252672
1220.040410	100483.983979	35.257690
1221.039251	100623.857864	35.262708
1222.479997	100813.101041	35.267725
1223.275134	100945.771239	35.272743
1224.532440	101117.514016	35.277760
1226.162612	101261.517850	35.282778
1227.305018	101414.527679	35.287796
1228.361428	101566.179199	35.292813
1229.839033	101721.966005	35.297831
1230.805792	101859.884712	35.302848
1232.098625	102029.850654	35.307866
1233.463126	102170.998160	35.312884
1234.656784	102311.990190	35.317901
1235.592055	102477.277060	35.322919
1236.462200	102649.137016	35.327936
1238.218703	102810.935820	35.332954
1239.207619	102969.175153	35.337972
1240.549853	103114.508086	35.342989
1241.626960	103299.279808	35.348007
1243.112505	103461.834891	35.353024
1244.390378	103628.087861	35.358042
1245.434942	103791.740425	35.363060
1246.918544	103948.654837	35.368077
1247.894491	104127.893362	35.373095
1249.215812	104290.840981	35.378112
1250.483341	104465.448004	35.383130
1251.524408	104631.391349	35.388148
1252.754608	104808.803815	35.393165
1254.001802	104993.258059	35.398183
1255.860846	105163.935073	35.403200
1256.769236	105330.024648	35.408218
1257.680433	105520.314028	35.413236
1259.491241	105665.847681	35.418253
1260.414475	105868.851409	35.423271
1261.926985	106031.717344	35.428288
1263.363686	106200.026210	35.433306
1264.264806	106380.932739	35.438324
1265.607451	106560.700935	35.443341
1267.134438	106735.125209	35.448359
1268.551477	106888.797827	35.453376
1269.844875	107088.221741	35.458394
1271.135325	107238.334723	35.463412
1272.460892	107420.599267	35.468429
1273.475814	107613.470963	35.473447
1275.116975	107772.752560	35.478464
1276.299718	107953.803406	35.483482
1277.574872	108132.765042	35.488500
1278.679575	108297.280789	35.493517
1279.911302	108479.618905	35.498535
1281.262919	108665.857018	35.503552
1282.699086	108827.292074	35.508570
1283.862657	108991.125975	35.513588
1285.096537	109191.931201	35.518605
1286.323851	109343.333166	35.523623
1287.405255	109555.646851	35.528640
1289.011453	109706.345266	35.533658
1290.157400	109903.163890	35.538676
1292.152695	110071.113546	35.543693
1293.036489	110240.893027	35.548711
1294.164383	110425.540865	35.553728
1295.883255	110556.573529	35.558746
1296.540256	110737.880626	35.563764
1298.211531	110895.310724	35.568781
1299.538832	111051.910357	35.573799
1300.267396	111212.036862	35.578816
1301.664198	111387.692675	35.583834
1302.409970	111550.837942	35.588852
1303.643758	111718.065422	35.593869
1305.401902	111910.416286	35.598887
1306.799451	112065.859171	35.603904
1307.952401	112246.769401	35.608922
1309.003891	112442.863810	35.613940
1310.620823	112614.233267	35.618957
1311.780712	112795.203374	35.623975
1313.067154	112973.116209	35.628992
1314.288191	113154.883149	35.634010
1315.848751	113348.675573	35.639028
1317.228842	113519.620489	35.644045
1318.435220	113702.014125	35.649063
1319.455022	113901.727048	35.654080
1321.016503	114058.966855	35.659098
1322.081524	114296.607729	35.664116
1323.751302	114450.040817	35.669133
1325.077762	114652.274855	35.674151
1326.251394	114850.381918	35.679168
1327.990935	115023.172839	35.684186
1329.000129	115227.335813	35.689204
1330.244434	115422.979830	35.694221
1331.811367	115606.817746	35.699239
1333.043688	115810.766385	35.704256
1334.580519	115997.581111	35.709274
1335.660543	116204.026185	35.714292
1337.275833	116388.951031	35.719309
1338.699533	116595.673883	35.724327
1339.743785	116787.700888	35.729344
1341.584147	116947.244249	35.734362
1342.719391	117177.784852	35.739380
1344.473571	117351.652994	35.744397
1345.629380	117542.414366	35.749415
1347.094746	117727.619689	35.754432
1348.704934	117905.041046	35.759450
1349.772223	118117.372847	35.764468
1351.629469	118298.594522	35.769485
1352.788241	118485.595210	35.774503
1353.817410	118656.117756	35.779520
1355.394770	118864.854310	35.784538
1356.356376	119036.916037	35.789556
1358.064339	119246.458042	35.794573
1358.828890	119444.843132	35.799591
1360.442541	119629.019165	35.804608
1361.913001	119806.165572	35.809626
1362.906012	120024.172890	35.814644
1364.353045	120212.109043	35.819661
1366.213927	120397.447982	35.824679
1367.328100	120595.311399	35.829696
1368.636694	120759.154728	35.834714
1369.884976	120947.564689	35.839732
1371.271386	121126.607757	35.844749
1372.483948	121304.818496	35.849767
1374.023027	121479.103211	35.854784
1375.606712	121662.576510	35.859802
1376.734165	121852.835893	35.864820
1378.095911	122043.376039	35.869837
1379.609200	122215.997991	35.874855
1380.841664	122407.511185	35.879872
1382.086379	122598.428564	35.884890
1383.088289	122782.800025	35.889908
1384.416104	122982.775229	35.894925
1386.061911	123171.986526	35.899943
1387.306958	123375.486147	35.904960
1389.040016	123546.448023	35.909978
1390.266597	123769.927136	35.914996
1391.696657	123969.234910	35.920013
1393.353502	124162.301887	35.925031
1394.378229	124363.627556	35.930048
1396.002873	124575.828171	35.935066
1397.289071	124779.040650	35.940084
1398.860906	124961.132728	35.945101
1399.983859	125171.555855	35.950119
1401.003853	125379.527044	35.955136
1402.931332	125577.488441	35.960154
1404.031120	125809.453263	35.965172
1405.653116	126001.728356	35.970189
1407.270533	126200.972270	35.975207
1408.712946	126430.785296	35.980224
1410.350482	126621.896975	35.985242
1411.256491	126838.042363	35.990260
1413.206824	127038.772250	35.995277
1414.453695	127233.763130	36.000295
1415.957321	127473.734390	36.005312
1417.440252	127663.991244	36.010330
1418.945764	127846.062603	36.015348
1420.261390	128089.894744	36.020365
1421.816616	128307.519393	36.025383
1423.231152	128478.309779	36.030400
1424.839717	128686.998142	36.035418
1425.787033	128909.461959	36.040436
1427.789722	129090.664489	36.045453
1428.802164	129334.606511	36.050471
1430.342166	129528.414310	36.055488
1431.888261	129726.643771	36.060506
1433.575296	129948.504343	36.065524
1434.561212	130152.843400	36.070541
1436.413180	130357.059017	36.075559
1437.524160	130566.372703	36.080576
1439.127596	130776.319169	36.085594
1440.513462	130971.048343	36.090612
1442.044523	131207.120302	36.095629
1443.404022	131391.075209	36.100647
1444.857069	131560.256797	36.105664
1446.588663	131794.148068	36.110682
1447.698698	131940.024193	36.115700
1449.239157	132160.760034	36.120717
1450.608889	132323.764068	36.125735
1451.813941	132530.708252	36.130752
1453.060459	132721.290704	36.135770
1454.313458	132935.515341	36.140788
1455.652908	133111.667367	36.145805
1457.204930	133347.867954	36.150823
1458.388252	133547.588424	36.155840
1460.072680	133752.919603	36.160858
1461.277145	133957.809038	36.165876
1462.639012	134195.491278	36.170893
1464.433495	134387.138164	36.175911
1465.938829	134629.844075	36.180928
1467.420935	134833.453947	36.185946
1468.607436	135042.763397	36.190964
1470.264517	135280.458405	36.195981
1472.037542	135477.539120	36.200999
1472.855936	135701.470791	36.206016
1474.442904	135935.241627	36.211034
1476.399264	136148.846352	36.216052
1477.487616	136381.889049	36.221069
1479.432537	136578.215009	36.226087
1480.506574	136847.858900	36.231104
1482.112151	137042.442541	36.236122
1483.485148	137285.318463	36.241140
1485.059765	137501.477428	36.246157
1486.657523	137728.443488	36.251175
1488.414936	137957.603547	36.256192
1489.868468	138180.160794	36.261210
1491.352139	138409.735360	36.266228
1492.387074	138661.369530	36.271245
1494.423649	138870.964253	36.276263
1495.854681	139097.992697	36.281280
1497.261929	139346.836276	36.286298
1498.610166	139559.358553	36.291316
1500.154034	139806.308710	36.296333
1502.135437	140018.543584	36.301351
1503.297810	140256.902467	36.306368
1505.328946	140483.694068	36.311386
1507.106907	140705.686437	36.316404
1508.181825	140958.917822	36.321421
1510.338432	141156.812078	36.326439
1511.562881	141381.786915	36.331456
1512.826898	141615.603321	36.336474
1514.438952	141828.302557	36.341492
1515.686358	142055.737464	36.346509
1517.381031	142298.210300	36.351527
1518.742713	142509.306486	36.356544
1520.279528	142763.632938	36.361562
1522.026120	142941.794420	36.366580
1523.065811	143230.652124	36.371597
1524.983529	143424.087095	36.376615
1526.482896	143622.507430	36.381632
1527.910355	143875.998649	36.386650
1529.161496	144075.690778	36.391668
1530.895753	144263.443931	36.396685
1532.319997	144519.412529	36.401703
1533.831930	144724.340154	36.406720
1535.334477	144905.720529	36.411738
1536.793455	145156.859724	36.416756
1538.085841	145339.442129	36.421773
1539.587949	145586.635979	36.426791
1541.454081	145814.013108	36.431808
1542.812758	146035.667159	36.436826
1544.351459	146274.608947	36.441844
1545.858815	146484.847270	36.446861
1547.454690	146718.408905	36.451879
1549.047357	146944.468715	36.456896
1550.155399	147170.442345	36.461914
1552.154042	147396.238097	36.466932
1553.571458	147661.094044	36.471949
1555.112613	147878.561673	36.476967
1556.587579	148113.914834	36.481984
1558.069411	148354.389897	36.487002
1559.773617	148580.253537	36.492020
1561.446590	148815.669173	36.497037
1563.055358	149084.563080	36.502055
1564.720805	149306.660375	36.507072
1565.957244	149558.364367	36.512090
1568.020984	149778.905801	36.517108
1569.285386	150036.643310	36.522125
1571.188927	150272.514744	36.527143
1572.816685	150523.378138	36.532160
1574.061752	150766.482361	36.537178
1575.660584	150986.231155	36.542196
1577.233589	151268.079897	36.547213
1579.336850	151498.464525	36.552231
1580.824106	151729.303599	36.557248
1582.026662	152005.956317	36.562266
1583.865591	152217.295252	36.567284
1585.624711	152483.886117	36.572301
1587.304600	152706.904526	36.577319
1588.673259	152968.807064	36.582336
1590.189579	153232.044800	36.587354
1592.057673	153444.020889	36.592372
1593.401981	153706.947405	36.597389
1595.057045	153950.390442	36.602407
1596.362444	154189.250418	36.607424
1598.174178	154460.108856	36.612442
1600.148937	154695.417528	36.617460
1601.405340	154971.401798	36.622477
1603.028804	155174.235526	36.627495
1604.448880	155454.622739	36.632512
1606.437576	155698.114247	36.637530
1608.210542	155921.925489	36.642548
1609.676015	156196.250954	36.647565
1611.635615	156431.257177	36.652583
1613.273427	156623.104228	36.657600
1614.236755	156887.003681	36.662618
1616.158034	157086.555583	36.667636
1617.620765	157334.187188	36.672653
1619.329449	157550.233952	36.677671
1620.570018	157766.204264	36.682688
1621.795552	158029.157915	36.687706
1623.940502	158238.495371	36.692724
1624.922267	158503.748420	36.697741
1627.058325	158732.224763	36.702759
1628.152130	158976.591841	36.707776
1629.537983	159212.570489	36.712794
1631.335967	159493.881793	36.717812
1632.862041	159717.148316	36.722829
1634.446394	160006.562589	36.727847
1636.334727	160233.579112	36.732864
1638.160649	160513.651454	36.737882
1639.650265	160764.384734	36.742900
1641.005073	161004.197379	36.747917
1642.596458	161287.470715	36.752935
1644.347254	161536.392620	36.757952
1645.877003	161803.967703	36.762970
1647.527961	162088.873875	36.767988
1648.807383	162345.675435	36.773005
1651.459055	162598.012548	36.778023
1652.581271	162898.315958	36.783040
1654.529072	163157.857922	36.788058
1655.823145	163431.037262	36.793076
1657.808235	163685.643805	36.798093
1659.004919	163978.043432	36.803111
1661.198606	164244.186937	36.808128
1662.732468	164512.694633	36.813146
1664.660425	164807.521276	36.818164
1666.456348	165058.045662	36.823181
1668.005604	165338.072749	36.828199
1669.586136	165616.029713	36.833216
1671.786907	165880.421094	36.838234
1673.410653	166147.569416	36.843252
1674.837990	166435.665182	36.848269
1676.842218	166681.614314	36.853287
1678.380314	166978.143660	36.858304
1679.758752	167240.544534	36.863322
1681.690399	167504.153112	36.868340
1683.561690	167801.561969	36.873357
1685.164013	168070.401688	36.878375
1686.754742	168330.785150	36.883392
1688.368675	168627.391584	36.888410
1690.529726	168896.655816	36.893428
1691.495270	169176.233592	36.898445
1693.342353	169433.628558	36.903463
1695.104069	169736.650993	36.908480
1696.678295	169989.983368	36.913498
1698.548452	170296.303594	36.918516
1699.773768	170570.193086	36.923533
1701.755635	170822.743207	36.928551
1703.675473	171103.553420	36.933568
1705.377882	171355.821593	36.938586
1706.863921	171625.706846	36.943604
1708.674811	171857.640053	36.948621
1710.216155	172154.868719	36.953639
1712.192269	172379.167823	36.958656
1713.173254	172674.738870	36.963674
1715.341275	172916.757043	36.968692
1716.979000	173209.576620	36.973709
1718.528994	173452.913994	36.978727
1720.285695	173729.367099	36.983744
1721.881518	174026.207957	36.988762
1723.677202	174261.050012	36.993780
1725.294751	174577.173654	36.998797
1726.882726	174832.019356	37.003815
1728.532934	175137.828675	37.008832
1729.923265	175393.064512	37.013850
1731.970726	175710.841399	37.018868
1733.766276	175983.980104	37.023885
1735.421682	176278.341610	37.028903
1736.942909	176601.017087	37.033920
1738.486047	176863.837012	37.038938
1740.970067	177142.303948	37.043956
1742.684539	177480.154102	37.048973
1744.147695	177765.587355	37.053991
1746.955048	178023.583316	37.059008
1748.135782	178358.379049	37.064026
1749.672480	178623.114210	37.069044
1751.342689	178940.087833	37.074061
1753.392711	179215.453128	37.079079
1755.056793	179540.552030	37.084096
1756.932979	179826.758455	37.089114
1758.813544	180110.720448	37.094132
1760.495377	180429.530404	37.099149
1762.315617	180735.455544	37.104167
1764.307365	181023.669010	37.109184
1766.258338	181345.158236	37.114202
1767.686235	181634.810225	37.119220
1770.014191	181913.511137	37.124237
1771.649153	182225.363503	37.129255
1773.392055	182519.602541	37.134272
1775.392434	182804.959011	37.139290
1777.317566	183108.765381	37.144308
1779.288584	183396.490396	37.149325
1780.796312	183681.537445	37.154343
1782.976700	183973.737400	37.159360
1784.910298	184270.495616	37.164378
1786.474169	184536.404814	37.169396
1788.357088	184830.560943	37.174413
1790.415005	185125.985495	37.179431
1792.178169	185399.887567	37.184448
1793.418862	185680.599433	37.189466
1795.497903	185993.207284	37.194484
1797.344021	186262.622172	37.199501
1798.557213	186535.412965	37.204519
1800.660834	186829.547108	37.209536
1802.305326	187098.440621	37.214554
1803.868324	187348.022548	37.219572
1805.807288	187616.682014	37.224589
1807.203650	187908.295918	37.229607
1809.691904	188161.402688	37.234624
1810.907712	188447.820489	37.239642
1812.846153	188716.207249	37.244660
1814.281028	189019.154069	37.249677
1815.772990	189294.010754	37.254695
1817.652082	189566.739112	37.259712
1819.452609	189884.024041	37.264730
1821.396126	190157.354715	37.269748
1822.944974	190475.343448	37.274765
1824.578712	190761.011018	37.279783
1826.582187	191059.768959	37.284800
1828.105647	191383.415036	37.289818
1830.254783	191688.270627	37.294836
1831.698455	191966.424592	37.299853
1833.371729	192317.845863	37.304871
1835.564662	192596.239851	37.309888
1837.252210	192942.269726	37.314906
1839.413078	193248.237347	37.319924
1841.366312	193575.675178	37.324941
1842.891475	193879.031709	37.329959
1845.245022	194214.367627	37.334976
1846.630059	194525.745875	37.339994
1849.110359	194843.082201	37.345012
1850.521316	195141.349871	37.350029
1852.159691	195482.087476	37.355047
1854.131683	195799.447048	37.360064
1856.500342	196125.896430	37.365082
1858.194997	196451.071464	37.370100
1860.701283	196766.055024	37.375117
1862.189179	197064.765973	37.380135
1864.676105	197392.435776	37.385152
1866.767545	197708.683994	37.390170
1868.396598	198007.365282	37.395188
1870.977954	198300.261742	37.400205
1872.563997	198644.315890	37.405223
1874.470026	198934.771897	37.410240
1876.404553	199247.335405	37.415258
1878.260873	199541.128077	37.420276
1880.430063	199854.889099	37.425293
1881.972604	200178.689859	37.430311
1884.212250	200446.076470	37.435328
1885.962071	200788.328777	37.440346
1888.013855	201068.301582	37.445364
1890.059542	201382.421114	37.450381
1891.603401	201685.782162	37.455399
1893.758772	201989.162079	37.460416
1895.111967	202298.116388	37.465434
1897.011990	202598.849210	37.470452
1898.489507	202914.006958	37.475469
1900.413718	203215.462799	37.480487
1902.430548	203518.327244	37.485504
1904.298691	203802.912728	37.490522
1905.924288	204112.608151	37.495540
1907.866532	204386.928323	37.500557
1909.406660	204677.663253	37.505575
1911.160915	204997.003058	37.510592
1913.332805	205292.058319	37.515610
1914.889339	205597.202928	37.520628
1916.703099	205889.284207	37.525645
1918.286037	206237.778267	37.530663
1920.684461	206528.538637	37.535680
1922.439554	206861.166716	37.540698
1924.052824	207184.336496	37.545716
1926.104366	207491.786272	37.550733
1927.680137	207822.747156	37.555751
1929.885328	208157.938836	37.560768
1931.830980	208481.773796	37.565786
1933.595305	208816.213950	37.570804
1935.773313	209151.110788	37.575821
1937.293029	209475.831109	37.580839
1939.402935	209824.503646	37.585856
1941.624094	210171.268951	37.590874
1943.511175	210496.494938	37.595892
1945.563012	210849.397218	37.600909
1947.866125	211183.447352	37.605927
1949.776332	211512.331166	37.610944
1951.790730	211849.388636	37.615962
1953.531158	212203.096932	37.620980
1955.865724	212524.542630	37.625997
1957.656250	212863.367556	37.631015
1959.415362	213223.718263	37.636032
1962.012951	213549.710440	37.641050
1964.275405	213879.947010	37.646068
1966.407674	214218.483549	37.651085
1968.789706	214575.340389	37.656103
1970.342462	214901.657404	37.661120
1972.437586	215226.379136	37.666138
1974.084011	215550.132561	37.671156
1976.255104	215906.598310	37.676173
1978.122575	216236.896529	37.681191
1980.237117	216564.744863	37.686208
1982.219884	216905.134209	37.691226
1983.929348	217254.849630	37.696244
1986.127376	217581.978558	37.701261
1988.142715	217906.751071	37.706279
1989.874151	218267.463220	37.711296
1992.415409	218580.309535	37.716314
1994.011715	218930.686087	37.721332
1996.239513	219268.343633	37.726349
1998.124651	219614.030705	37.731367
2000.137444	219940.488872	37.736384
2002.257034	220287.411639	37.741402
2003.955872	220636.891409	37.746420
2006.242349	220981.086527	37.751437
2008.215037	221308.814148	37.756455
2010.007141	221639.644563	37.761472
2011.991339	221949.406743	37.766490
2013.852318	222261.183209	37.771508
2015.950640	222574.777105	37.776525
2018.004169	222895.337532	37.781543
2019.725567	223225.919438	37.786560
2021.710619	223550.188394	37.791578
2023.500611	223902.576503	37.796596
2025.103189	224265.268250	37.801613
2027.268104	224601.436030	37.806631
2029.204761	224940.752374	37.811648
2031.143703	225282.253805	37.816666
2033.356122	225636.817399	37.821684
2035.094144	225971.801574	37.826701
2037.172695	226330.859069	37.831719
2039.242818	226688.433814	37.836736
2041.440068	227035.729963	37.841754
2043.161043	227397.350319	37.846772
2045.520542	227750.896534	37.851789
2047.320199	228106.006027	37.856807
2049.175877	228473.958693	37.861824
2051.405853	228839.771045	37.866842
2053.555234	229202.702515	37.871860
2055.814594	229580.119582	37.876877
2057.926957	229950.729840	37.881895
2059.890424	230304.958848	37.886912
2062.242607	230671.343574	37.891930
2063.856105	231038.862856	37.896948
2066.211971	231413.478683	37.901965
2068.746903	231777.578534	37.906983
2070.786125	232155.447683	37.912000
2073.201927	232522.845635	37.917018
2075.305807	232888.745250	37.922036
2077.589694	233243.950674	37.927053
2079.578904	233611.953879	37.932071
2081.726789	233958.649854	37.937088
2084.140313	234332.328430	37.942106
2086.143919	234697.361899	37.947124
2088.381508	235052.708282	37.952141
2090.670274	235419.578646	37.957159
2092.415884	235776.123162	37.962176
2094.651470	236134.064324	37.967194
2096.745526	236499.877348	37.972212
2098.874695	236848.643596	37.977229
2100.845191	237227.508298	37.982247
2103.001450	237582.647781	37.987264
2105.280224	237949.528722	37.992282
2107.101877	238310.082875	37.997300
2109.287380	238678.352639	38.002317
2111.600978	239029.382686	38.007335
2113.763766	239404.186077	38.012352
2115.281778	239774.952903	38.017370
2117.343839	240140.630971	38.022388
2119.798004	240506.756013	38.027405
2122.010515	240864.970481	38.032423
2124.153435	241209.786069	38.037440
2126.140813	241540.073294	38.042458
2128.133913	241882.908038	38.047476
2130.095213	242229.152392	38.052493
2132.293248	242562.279217	38.057511
2134.362041	242913.232865	38.062528
2136.681780	243253.835275	38.067546
2138.591381	243597.069081	38.072564
2140.636080	243952.322105	38.077581
2142.373469	244300.690579	38.082599
2144.332209	244662.385483	38.087616
2146.608308	245026.444103	38.092634
2148.626455	245397.859987	38.097652
2150.706032	245765.914286	38.102669
2152.628627	246132.775255	38.107687
2154.216630	246522.830329	38.112704
2156.557413	246902.505197	38.117722
2158.424987	247291.857665	38.122740
2161.004908	247686.686432	38.127757
2162.939165	248074.125384	38.132775
2165.049303	248479.089607	38.137792
2167.599203	248859.219089	38.142810
2169.544991	249272.949520	38.147828
2171.644465	249671.212727	38.152845
2173.917156	250073.005675	38.157863
2175.924912	250485.180033	38.162880
2178.284348	250887.697929	38.167898
2180.537088	251299.987929	38.172916
2182.963536	251708.237960	38.177933
2184.932454	252123.445387	38.182951
2187.267311	252538.570390	38.187968
2189.530259	252951.853458	38.192986
2191.746495	253356.254259	38.198004
2194.200744	253778.170928	38.203021
2196.474933	254188.330617	38.208039
2198.807212	254595.255941	38.213056
2201.018961	255004.233412	38.218074
2202.985302	255420.083824	38.223092
2205.480533	255826.985888	38.228109
2208.189726	256231.213015	38.233127
2209.976139	256656.366305	38.238144
2212.556082	257053.502890	38.243162
2214.831147	257461.636965	38.248180
2216.698360	257871.055785	38.253197
2219.468102	258283.609154	38.258215
2221.473085	258698.088105	38.263232
2223.673956	259101.156387	38.268250
2226.102093	259501.979283	38.273268
2228.254639	259926.064519	38.278285
2230.548967	260319.187545	38.283303
2232.271295	260735.442107	38.288320
2235.169945	261142.645244	38.293338
2237.313487	261543.872051	38.298356
2239.417811	261944.140341	38.303373
2241.799454	262344.873268	38.308391
2244.060379	262738.538472	38.313408
2246.242673	263111.208446	38.318426
2248.278533	263493.326565	38.323444
2250.255183	263864.886888	38.328461
2253.050884	264239.924983	38.333479
2255.010870	264624.393493	38.338496
2257.235742	265007.016802	38.343514
2259.257045	265400.265862	38.348532
2261.302479	265786.297019	38.353549
2263.852482	266170.673557	38.358567
2265.962053	266568.710963	38.363584
2267.939077	266967.582651	38.368602
2270.274870	267367.617163	38.373620
2272.443839	267766.205077	38.378637
2274.406883	268178.950156	38.383655
2276.842416	268582.627901	38.388672
2279.173563	268996.204364	38.393690
2281.639101	269408.794489	38.398708
2283.418920	269838.234379	38.403725
2285.947890	270249.595633	38.408743
2287.963931	270672.774783	38.413760
2290.795319	271091.074480	38.418778
2293.025462	271520.977427	38.423796
2295.201571	271957.392406	38.428813
2297.765076	272374.160155	38.433831
2299.751428	272810.224516	38.438848
2302.307668	273226.307823	38.443866
2304.865536	273660.579826	38.448884
2307.229418	274092.113718	38.453901
2309.497428	274516.245102	38.458919
2311.875722	274954.762803	38.463936
2314.010191	275378.127965	38.468954
2316.364632	275821.755612	38.473972
2319.019049	276251.109802	38.478989
2321.499263	276688.874724	38.484007
2323.497145	277134.286293	38.489024
2325.855297	277568.844247	38.494042
2328.536788	278004.265395	38.499060
2330.629204	278430.710818	38.504077
2332.946062	278861.337518	38.509095
2335.380121	279309.626264	38.514112
2338.039545	279744.516949	38.519130
2340.247125	280181.308129	38.524148
2342.472541	280618.578951	38.529165
2345.274106	281040.389209	38.534183
2347.383632	281475.671095	38.539200
2349.926956	281922.874325	38.544218
2352.427115	282351.996965	38.549236
2354.592858	282788.361455	38.554253
2357.099309	283217.457098	38.559271
2359.545852	283644.478848	38.564288
2361.865630	284090.267921	38.569306
2364.458326	284519.272640	38.574324
2366.662405	284948.414783	38.579341
2369.251229	285361.618575	38.584359
2371.740548	285775.980889	38.589376
2373.734687	286174.137897	38.594394
2376.366220	286567.773349	38.599412
2378.699813	286961.328610	38.604429
2380.655733	287353.952598	38.609447
2383.242261	287757.374089	38.614464
2385.520952	288161.961633	38.619482
2387.738084	288560.080702	38.624500
2389.648659	288977.350845	38.629517
2392.363832	289382.655180	38.634535
2394.369502	289794.447537	38.639552
2396.660602	290224.230061	38.644570
2398.922929	290652.136698	38.649588
2401.515482	291066.374490	38.654605
2404.082778	291495.882656	38.659623
2406.302540	291939.213425	38.664640
2408.592663	292365.842781	38.669658
2411.132317	292803.151730	38.674676
2413.370599	293252.319813	38.679693
2415.854832	293672.057441	38.684711
2418.378801	294138.985655	38.689728
2421.074366	294576.241177	38.694746
2423.775203	295018.702463	38.699764
2426.119872	295461.168479	38.704781
2428.422949	295898.712131	38.709799
2431.200367	296338.338858	38.714816
2433.359871	296775.166713	38.719834
2435.962567	297223.227256	38.724852
2438.307254	297681.640837	38.729869
2441.193257	298121.220923	38.734887
2443.681800	298583.368970	38.739904
2445.897440	299022.240265	38.744922
2448.676314	299465.898343	38.749940
2451.169582	299931.115735	38.754957
2453.438633	300369.162315	38.759975
2456.068515	300812.281673	38.764992
2458.097847	301262.302588	38.770010
2461.086504	301713.719711	38.775028
2463.215863	302173.349329	38.780045
2466.016367	302614.810980	38.785063
2468.555423	303079.250016	38.790080
2470.758541	303531.573750	38.795098
2473.579891	303971.681872	38.800116
2476.105313	304430.810032	38.805133
2478.767754	304890.905644	38.810151
2481.095994	305348.080830	38.815168
2483.242393	305791.820983	38.820186
2485.943104	306249.111969	38.825204
2488.334796	306700.887666	38.830221
2490.937394	307162.178958	38.835239
2493.865790	307621.867583	38.840256
2495.928834	308072.395211	38.845274
2498.175008	308513.341782	38.850292
2500.717528	308986.701086	38.855309
2503.205196	309425.878962	38.860327
2505.662419	309875.677217	38.865344
2508.183347	310295.212598	38.870362
2510.777125	310722.456455	38.875380
2513.113241	311142.449908	38.880397
2515.892561	311554.726377	38.885415
2518.382233	311992.599040	38.890432
2521.176642	312420.287414	38.895450
2523.485725	312834.716478	38.900468
2525.890735	313264.977828	38.905485
2528.372897	313705.181668	38.910503
2530.832909	314132.814779	38.915520
2533.213597	314568.306973	38.920538
2535.783959	315014.993540	38.925556
2537.943386	315463.013234	38.930573
2540.241845	315909.027881	38.935591
2542.657716	316364.571757	38.940608
2545.269005	316823.257399	38.945626
2547.834702	317281.160818	38.950644
2550.342147	317768.075847	38.955661
2552.893876	318213.582919	38.960679
2555.504229	318685.898670	38.965696
2558.448096	319156.406815	38.970714
2560.875147	319624.937299	38.975732
2563.179257	320108.672535	38.980749
2566.202152	320582.157876	38.985767
2568.803103	321056.672704	38.990784
2570.944218	321541.492867	38.995802
2573.861223	322015.800191	39.000820
2576.333110	322496.219905	39.005837
2578.827468	322979.528635	39.010855
2581.380976	323475.752072	39.015872
2584.208698	323960.780251	39.020890
2586.867059	324434.505828	39.025908
2589.356732	324922.756561	39.030925
2592.206497	325410.287101	39.035943
2595.310240	325897.342804	39.040960
2597.448181	326384.599390	39.045978
2600.591960	326856.812029	39.050996
2603.135303	327359.159534	39.056013
2605.679462	327834.737354	39.061031
2608.559348	328315.338098	39.066048
2611.183468	328809.283237	39.071066
2613.818746	329292.659309	39.076084
2616.419495	329775.326754	39.081101
2619.225761	330253.514581	39.086119
2621.849853	330737.238740	39.091136
2624.191375	331217.373188	39.096154
2627.251441	331704.373982	39.101172
2629.547998	332194.057228	39.106189
2632.388997	332668.211737	39.111207
2634.811059	333152.256667	39.116224
2637.445122	333637.026527	39.121242
2640.222680	334126.341059	39.126260
2642.851736	334609.505271	39.131277
2645.566645	335086.431355	39.136295
2648.483803	335534.527157	39.141312
2651.061136	335986.330331	39.146330
2653.584755	336423.970248	39.151348
2655.701623	336889.171158	39.156365
2658.298762	337337.458071	39.161383
2660.936054	337790.001380	39.166400
2662.922407	338267.502816	39.171418
2665.647857	338715.404567	39.176436
2668.413702	339180.334192	39.181453
2671.134786	339673.172046	39.186471
2673.942436	340131.842034	39.191488
2675.995363	340604.466028	39.196506
2678.624086	341118.102061	39.201524
2681.585788	341587.451739	39.206541
2684.155407	342080.167832	39.211559
2686.775513	342576.502710	39.216576
2689.122811	343086.130043	39.221594
2692.114008	343579.960604	39.226612
2694.528990	344080.987297	39.231629
2697.065536	344587.982296	39.236647
2699.786129	345096.949520	39.241664
2702.515008	345617.843557	39.246682
2705.024816	346139.351582	39.251700
2708.000851	346663.015226	39.256717
2710.758826	347187.013302	39.261735
2713.574524	347716.201860	39.266752
2716.160031	348252.200320	39.271770
2719.382808	348780.781335	39.276788
2721.674667	349316.003773	39.281805
2724.309076	349845.099455	39.286823
2727.645403	350370.829479	39.291840
2730.127193	350913.723753	39.296858
2733.170683	351446.217072	39.301876
2735.944824	351983.520258	39.306893
2738.676379	352512.269997	39.311911
2741.489335	353046.002432	39.316928
2744.117792	353585.419480	39.321946
2747.516329	354123.439827	39.326964
2750.620640	354646.397643	39.331981
2752.942936	355197.751672	39.336999
2755.843986	355724.259118	39.342016
2758.490366	356264.533866	39.347034
2761.572998	356790.747704	39.352052
2764.233207	357325.906930	39.357069
2766.909263	357858.418146	39.362087
2770.099520	358398.939195	39.367104
2772.522322	358932.494275	39.372122
2775.727531	359463.102305	39.377140
2778.522564	359987.170335	39.382157
2780.861669	360522.675663	39.387175
2784.006433	361051.981444	39.392192
2786.960551	361584.331855	39.397210
2789.429639	362119.621087	39.402228
2792.293007	362646.390282	39.407245
2795.147327	363175.083869	39.412263
2798.087022	363685.281701	39.417280
2800.623813	364177.797656	39.422298
2803.632391	364659.549131	39.427316
2806.052153	365162.478454	39.432333
2808.562136	365657.698306	39.437351
2811.177805	366156.829636	39.442368
2813.611161	366660.679213	39.447386
2816.526658	367173.811119	39.452404
2819.592152	367679.452473	39.457421
2822.180734	368208.104341	39.462439
2824.947061	368724.134926	39.467456
2827.377026	369251.708185	39.472474
2830.081464	369780.957189	39.477492
2833.032065	370314.119384	39.482509
2835.646592	370854.610943	39.487527
2838.641766	371402.444960	39.492544
2841.726829	371951.907074	39.497562
2844.125783	372506.342582	39.502580
2847.012843	373056.811298	39.507597
2850.271188	373607.594620	39.512615
2852.974293	374155.312263	39.517632
2855.909340	374722.294870	39.522650
2858.946452	375281.235744	39.527668
2861.711947	375833.640550	39.532685
2864.608204	376394.618294	39.537703
2867.603297	376956.206924	39.542720
2870.505211	377523.231947	39.547738
2873.502901	378088.001145	39.552756
2876.461277	378654.848958	39.557773
2879.492802	379227.436132	39.562791
2882.606166	379787.596169	39.567808
2885.535831	380351.329015	39.572826
2888.500946	380914.058706	39.577844
2891.841009	381482.378119	39.582861
2894.073996	382048.149981	39.587879
2897.707365	382620.668045	39.592896
2900.513763	383185.748862	39.597914
2903.597120	383754.633254	39.602932
2906.437567	384309.671840	39.607949
2909.486824	384880.979839	39.612967
2912.303018	385427.888419	39.617984
2914.963210	386006.470098	39.623002
2918.210946	386581.144929	39.628020
2921.419180	387144.402810	39.633037
2924.080432	387709.793128	39.638055
2927.003160	388272.444682	39.643072
2929.845476	388851.814948	39.648090
2932.857041	389426.025717	39.653108
2936.079305	389975.515789	39.658125
2938.775831	390547.475754	39.663143
2941.867334	391124.943666	39.668160
2944.878245	391673.046001	39.673178
2947.508479	392260.560839	39.678196
2950.963519	392835.711317	39.683213
2953.501421	393387.919391	39.688231
2956.541403	393914.349413	39.693248
2959.463084	394450.984732	39.698266
2961.946689	394974.849173	39.703284
2964.914311	395499.719417	39.708301
2967.725710	396040.861118	39.713319
2971.036040	396573.623101	39.718336
2973.723071	397102.291281	39.723354
2976.358174	397663.366022	39.728372
2979.399757	398185.114524	39.733389
2982.344445	398754.160061	39.738407
2984.982095	399282.218294	39.743424
2988.143485	399875.932388	39.748442
2990.718527	400411.944058	39.753460
2993.772091	400976.877080	39.758477
2996.643399	401573.674152	39.763495
2999.169324	402144.907492	39.768512
3002.620265	402727.266589	39.773530
3005.275718	403318.031401	39.778548
3008.548382	403923.214565	39.783565
3011.106760	404503.958522	39.788583
3014.053031	405108.156632	39.793600
3017.225743	405717.859183	39.798618
3020.157308	406337.677527	39.803636
3023.339735	406931.029143	39.808653
3026.263063	407555.412877	39.813671
3029.292406	408170.971110	39.818688
3032.606344	408789.843333	39.823706
3035.121741	409423.353779	39.828724
3038.473467	410027.847968	39.833741
3041.691219	410694.425925	39.838759
3044.700621	411294.411858	39.843776
3048.002006	411941.736377	39.848794
3051.161601	412570.187050	39.853812
3054.239018	413189.741427	39.858829
3057.376847	413835.124407	39.863847
3060.830861	414449.853388	39.868864
3064.162996	415093.277223	39.873882
3067.261832	415707.225003	39.878900
3070.122118	416342.890366	39.883917
3073.582799	416976.292741	39.888935
3076.592653	417595.637604	39.893952
3079.694428	418235.100162	39.898970
3083.090193	418854.407394	39.903988
3086.431118	419479.816571	39.909005
3089.190592	420109.028705	39.914023
3092.637001	420719.114486	39.919040
3095.850160	421359.781040	39.924058
3098.619846	421990.165556	39.929076
3101.830384	422608.709922	39.934093
3104.836658	423237.711162	39.939111
3107.534970	423859.906238	39.944128
3111.020533	424493.008600	39.949146
3114.255195	425116.281008	39.954164
3117.341037	425742.501373	39.959181
3120.494352	426353.800803	39.964199
3123.448397	426953.515664	39.969216
3126.761158	427545.535507	39.974234
3129.823123	428128.133355	39.979252
3132.864925	428696.232469	39.984269
3135.857322	429288.492266	39.989287
3138.430459	429873.712831	39.994304
3141.367075	430477.302462	39.999322
3144.562520	431073.416029	40.004340
3147.339189	431672.393647	40.009357
3150.448057	432302.052283	40.014375
3153.658879	432906.606094	40.019392
3156.723074	433513.853521	40.024410
3159.357006	434156.990236	40.029428
3162.581248	434770.438025	40.034445
3165.691207	435426.661769	40.039463
3168.807957	436070.838813	40.044480
3171.973737	436698.582460	40.049498
3174.938390	437335.635579	40.054516
3178.145806	438021.656808	40.059533
3181.645835	438677.379760	40.064551
3184.280345	439337.450837	40.069568
3187.399761	440022.266159	40.074586
3190.855430	440689.134191	40.079604
3194.124794	441356.013613	40.084621
3197.189356	442030.198716	40.089639
3200.442942	442733.804022	40.094656
3203.464131	443395.502333	40.099674
3206.760061	444114.301151	40.104692
3210.339754	444780.531186	40.109709
3213.417397	445504.588406	40.114727
3216.858923	446168.928435	40.119744
3220.274162	446879.525167	40.124762
3223.296067	447570.419720	40.129780
3226.763610	448269.221814	40.134797
3230.042542	448965.805665	40.139815
3233.121213	449660.223851	40.144832
3236.447629	450381.814252	40.149850
3239.853520	451074.164406	40.154868
3243.083984	451785.096972	40.159885
3246.446281	452504.236587	40.164903
3249.933052	453176.822425	40.169920
3253.032155	453918.936625	40.174938
3256.192343	454605.044677	40.179956
3259.614029	455337.749622	40.184973
3263.488290	456028.509138	40.189991
3266.608021	456727.362038	40.195008
3269.715270	457453.418714	40.200026
3273.484540	458163.711696	40.205044
3276.401966	458852.359399	40.210061
3279.723423	459563.234920	40.215079
3282.862254	460286.562761	40.220096
3286.834138	460974.370248	40.225114
3289.618690	461687.740929	40.230132
3292.833806	462391.357444	40.235149
3296.236620	463085.815524	40.240167
3299.031375	463755.812780	40.245184
3302.681945	464427.525519	40.250202
3305.839256	465076.684257	40.255220
3308.971339	465733.414613	40.260237
3312.130737	466416.725841	40.265255
3315.328413	467053.476264	40.270272
3318.681057	467763.368686	40.275290
3321.081534	468429.133939	40.280308
3324.527446	469109.783899	40.285325
3328.066765	469804.860685	40.290343
3331.105996	470507.680126	40.295360
3334.430570	471192.933754	40.300378
3337.613566	471900.588445	40.305396
3340.587970	472627.871294	40.310413
3343.945286	473331.151149	40.315431
3347.015101	474056.750182	40.320448
3350.452678	474790.759372	40.325466
3353.685588	475540.953086	40.330484
3356.383047	476269.363216	40.335501
3360.509260	476986.550757	40.340519
3363.428688	477779.176690	40.345536
3367.165700	478505.774207	40.350554
3370.273179	479289.615692	40.355572
3373.521178	480038.526594	40.360589
3377.469652	480777.037732	40.365607
3380.032959	481588.269594	40.370624
3383.945202	482369.435479	40.375642
3387.356986	483122.802244	40.380660
3390.902331	483934.792274	40.385677
3394.353663	484710.883390	40.390695
3397.650620	485464.581643	40.395712
3401.177310	486265.713154	40.400730
3404.455155	487038.604938	40.405748
3408.413776	487820.503182	40.410765
3411.641554	488638.761523	40.415783
3415.312309	489407.705636	40.420800
3418.809297	490210.646161	40.425818
3422.609077	490967.381356	40.430836
3425.648580	491779.167848	40.435853
3429.574427	492577.847368	40.440871
3432.878657	493345.930153	40.445888
3436.819709	494157.773424	40.450906
3440.225016	494922.037077	40.455924
3443.844113	495732.245644	40.460941
3447.129395	496480.604712	40.465959
3450.860013	497280.626421	40.470976
3454.325102	498051.769551	40.475994
3457.781702	498861.713225	40.481012
3461.301924	499615.662618	40.486029
3465.155367	500396.288751	40.491047
3468.537178	501168.473100	40.496064
3471.889923	501974.152705	40.501082
3475.404797	502726.154397	40.506100
3478.460667	503529.740513	40.511117
3482.110783	504291.067181	40.516122
3484.835043	505009.695107	40.521127
3488.404700	505668.343264	40.526132
3492.121072	506272.594058	40.531136
3494.470532	506888.476250	40.536141
3497.361451	507373.952628	40.541146
3499.849453	507778.822342	40.546151
3502.610267	508203.676748	40.551156
3504.535836	508529.379422	40.556160
3507.109944	508778.773894	40.561165
3509.169630	509044.538192	40.566170
3510.507411	509231.685127	40.571175
3512.591847	509334.520816	40.576180
3514.145274	509396.811578	40.581184
3515.207572	509447.036825	40.586189
3516.293019	509509.502330	40.591194
3517.199699	509474.498821	40.596199
3518.149905	509426.535913	40.601204
3518.833611	509346.537306	40.606208
3519.035653	509255.230348	40.611213
3520.370656	509113.704042	40.616218
3520.290490	508989.552560	40.621223
3521.072153	508857.016641	40.626228
3521.795168	508668.274968	40.631232
3521.590415	508492.580426	40.636237
3522.151173	508290.451735	40.641242
3522.112027	508093.424842	40.646247
3522.047696	507854.452239	40.651252
3521.929853	507610.778926	40.656256
3522.238538	507418.445881	40.661261
3522.477816	507188.726796	40.666266
3522.203111	506925.384462	40.671271
3522.062560	506665.660406	40.676276
3522.149954	506444.052085	40.681280
3521.909443	506174.316880	40.686285
3521.754885	505963.570174	40.691290
3521.232612	505694.378157	40.696295
3521.814441	505411.748427	40.701300
3521.346818	505191.578368	40.706304
3521.014111	504958.732102	40.711309
3520.859926	504666.692309	40.716314
3520.715991	504422.826886	40.721319
3520.234792	504178.454674	40.726324
3520.579103	503901.860922	40.731328
3520.104240	503673.119674	40.736333
3519.645076	503465.377307	40.741338
3519.080551	503202.834771	40.746343
3519.384166	502936.810599	40.751348
3518.699827	502718.314212	40.756352
3518.375030	502526.483302	40.761357
3518.552912	502274.995725	40.766362
3518.479080	502030.883828	40.771367
3517.901429	501845.007709	40.776372
3517.797755	501619.623327	40.781376
3517.086594	501394.483966	40.786381
3516.673873	501179.469081	40.791386
3516.801679	500973.579003	40.796391
3516.840384	500743.757149	40.801396
3516.402576	500574.955449	40.806400
3515.745346	500407.502996	40.811405
3515.572389	500195.020098	40.816410
3515.797686	499987.736504	40.821415
3515.623783	499828.403134	40.826420
3515.391389	499659.307249	40.831424
3515.110743	499443.491340	40.836429
3514.873022	499283.100125	40.841434
3514.619390	499096.992437	40.846439
3514.427686	498934.363344	40.851444
3514.293154	498762.054169	40.856448
3513.597829	498597.476596	40.861453
3513.998105	498444.824223	40.866458
3513.288105	498299.332621	40.871463
3513.527772	498112.529313	40.876468
3512.982903	497991.816803	40.881472
3512.833658	497820.361679	40.886477
3512.619867	497681.115283	40.891482
3512.437679	497557.051669	40.896487
3512.116663	497392.960931	40.901492
3511.826868	497279.949753	40.906496
3512.113665	497121.380460	40.911501
3511.935167	496994.882160	40.916506
3511.419754	496916.586602	40.921511
3511.129356	496764.130543	40.926516
3511.787953	496636.940513	40.931520
3510.949513	496521.479745	40.936525
3511.003845	496405.472085	40.941530
3510.456511	496301.761324	40.946535
3510.919625	496166.143214	40.951540
3510.715468	496092.402561	40.956544
3509.905069	495974.199693	40.961549
3510.873375	495831.815596	40.966554
3510.289675	495764.918597	40.971559
3509.860187	495647.261031	40.976564
3509.991261	495568.857526	40.981568
3509.776527	495456.278925	40.986573
3509.758536	495380.480574	40.991578
3509.746671	495256.931420	40.996583
3509.475730	495197.983382	41.001588
3509.612694	495073.447390	41.006592
3508.927162	494987.423108	41.011597
3509.258449	494936.126443	41.016602
3508.633046	494843.509211	41.021607
3509.087950	494736.086610	41.026612
3508.771559	494689.246426	41.031616
3508.710708	494594.513220	41.036621
3509.333755	494499.722076	41.041626
3508.525140	494457.668424	41.046631
3508.632074	494337.638989	41.051636
3508.658010	494296.820306	41.056640
3508.153160	494212.637472	41.061645
3508.435697	494145.648313	41.066650
3508.330843	494050.109046	41.071655
3508.277032	494012.188769	41.076660
3508.246312	493920.992092	41.081664
3507.923105	493871.872134	41.086669
3508.382746	493774.925598	41.091674
3507.869720	493753.585966	41.096679
3507.800752	493643.403976	41.101684
3507.743828	493598.849469	41.106688
3507.479771	493561.012136	41.111693
3507.363866	493471.497845	41.116698
3507.576739	493423.659269	41.121703
3507.090572	493383.071430	41.126708
3507.543156	493291.136935	41.131712
3507.128592	493281.428672	41.136717
3507.376702	493205.427413	41.141722
3507.143575	493164.242046	41.146727
3506.780506	493103.630712	41.151732
3507.604051	493036.754608	41.156736
3506.812499	493042.652862	41.161741
3506.727122	492971.210480	41.166746
3506.582063	492915.780210	41.171751
3507.203383	492863.317835	41.176756
3506.724497	492841.971755	41.181760
3506.862665	492765.429007	41.186765
3506.707571	492741.600790	41.191770
3506.266717	492699.839511	41.196775
3506.940898	492622.147958	41.201780
3506.920113	492621.847357	41.206784
3506.715318	492591.341921	41.211789
3506.607924	492535.600706	41.216794
3506.809558	492487.761500	41.221799
3506.312457	492460.593868	41.226804
3506.426620	492428.619736	41.231808
3505.874693	492374.163742	41.236813
3506.296243	492293.927920	41.241818
3505.975282	492288.711651	41.246823
3506.250159	492268.005439	41.251828
3506.408461	492256.180336	41.256832
3506.167281	492207.650737	41.261837
3505.716788	492167.257179	41.266842
3505.902040	492131.624914	41.271847
3506.067181	492075.383450	41.276852
3506.632808	492027.840047	41.281856
3505.358903	492028.649096	41.286861
3505.375169	492000.589340	41.291866
3505.429463	491972.928690	41.296871
3505.320910	491948.585655	41.301876
3506.206934	491921.350568	41.306880
3506.326596	491874.738224	41.311885
3506.048960	491849.915333	41.316890
3505.954158	491826.177706	41.321895
3505.887808	491797.168443	41.326900
3506.259689	491750.566572	41.331904
3505.799511	491740.611484	41.336909
3505.903071	491727.224690	41.341914
3505.695820	491720.622862	41.346919
3505.815301	491659.778624	41.351924
3505.896037	491605.929433	41.356928
3505.443066	491610.913640	41.361933
3505.368052	491597.554977	41.366938
3505.697005	491551.668437	41.371943
3505.407093	491503.195354	41.376948
3505.443712	491485.919220	41.381952
3505.400923	491476.708360	41.386957
3505.008612	491474.288676	41.391962
3505.390943	491442.118534	41.396967
3505.511380	491411.357179	41.401972
3505.970411	491376.490546	41.406976
3505.013289	491381.655787	41.411981
3505.364856	491353.845945	41.416986
3505.001872	491349.243811	41.421991
3504.929238	491317.145361	41.426996
3506.035354	491291.292680	41.432000
3505.845834	491252.780469	41.437005
3505.881128	491219.854447	41.442010
3505.427146	491223.218216	41.447015
3504.938922	491198.377095	41.452020
3505.622094	491157.498295	41.457024
3504.847480	491174.334201	41.462029
3505.076746	491155.254671	41.467034
3504.894883	491156.853444	41.472039
3505.195513	491124.239847	41.477044
3505.387988	491070.725987	41.482048
3504.540309	491102.413141	41.487053
3504.848502	491100.591753	41.492058
3505.142097	491051.518806	41.497063
3505.342115	491023.783076	41.502068
3505.737645	491025.847724	41.507072
3505.325428	491001.247566	41.512077
3505.117559	491008.826858	41.517082
3504.906838	490999.287772	41.522087
3505.076982	490972.670931	41.527092
3504.906761	490947.171446	41.532096
3504.909702	490921.644558	41.537101
3505.750132	490881.500019	41.542106
3505.527004	490872.469307	41.547111
3505.120520	490839.815032	41.552116
3505.364248	490823.417215	41.557120
3505.181061	490821.977352	41.562125
3505.204037	490846.183380	41.567130
3505.175704	490803.086462	41.572135
3504.955811	490773.390811	41.577140
3505.517478	490735.619828	41.582144
3505.092235	490739.586918	41.587149
3505.006789	490704.197315	41.592154
3505.119196	490675.512601	41.597159
3505.212251	490667.951267	41.602164
3505.398723	490643.711851	41.607168
3505.271581	490629.246472	41.612173
3505.200148	490596.589467	41.617178
3505.137643	490600.853794	41.622183
3505.030243	490627.106651	41.627188
3505.186145	490622.067787	41.632192
3504.736367	490585.013495	41.637197
3505.227798	490536.363772	41.642202
3505.139555	490558.815045	41.647207
3504.734555	490557.967353	41.652212
3504.459198	490529.698243	41.657216
3504.924776	490491.840662	41.662221
3505.129479	490525.742949	41.667226
3504.799703	490506.143333	41.672231
3504.580185	490473.357572	41.677236
3505.457847	490437.967195	41.682240
3504.960389	490423.965378	41.687245
3505.072805	490443.194188	41.692250
3505.198555	490437.805498	41.697255
3504.557277	490403.971999	41.702260
3504.648306	490387.496639	41.707264
3505.077280	490359.065304	41.712269
3504.806545	490326.945822	41.717274
3504.803272	490347.408597	41.722279
3504.663263	490370.729312	41.727284
3504.863453	490340.206844	41.732288
3504.557645	490317.716237	41.737293
3504.837911	490317.216070	41.742298
3504.815719	490320.309156	41.747303
3504.607284	490296.587552	41.752308
3504.628346	490281.440040	41.757312
3505.151430	490251.676785	41.762317
3505.010677	490253.421085	41.767322
3504.630959	490256.520039	41.772327
3505.247082	490194.883467	41.777332
3505.342923	490204.542363	41.782336
3504.745241	490219.426471	41.787341
3504.508163	490210.093747	41.792346
3504.513116	490198.544833	41.797351
3504.290510	490175.483761	41.802356
3504.173950	490145.618836	41.807360
3504.534512	490140.750096	41.812365
3504.888618	490128.639458	41.817370
3504.799140	490113.863831	41.822375
3504.645765	490122.751761	41.827380
3505.219986	490135.323423	41.832384
3504.592447	490107.159990	41.837389
3504.210863	490092.278564	41.842394
3504.822327	490061.032194	41.847399
3505.050594	490092.652289	41.852404
3504.949193	490110.446386	41.857408
3504.664724	490096.613261	41.862413
3504.902542	490079.709234	41.867418
3504.926353	490057.875318	41.872423
3504.597929	490031.183995	41.877428
3504.899219	490007.026913	41.882432
3504.746033	489994.185965	41.887437
3504.620589	489986.608242	41.892442
3504.879209	489960.887689	41.897447
3504.868904	489990.114452	41.902452
3504.937423	489973.692939	41.907456
3504.334263	489957.782772	41.912461
3504.612927	489938.896803	41.917466
3504.895837	489933.128578	41.922471
3504.964143	489902.524945	41.927476
3504.959919	489885.962902	41.932480
3504.774308	489914.052529	41.937485
3504.838615	489904.013565	41.942490
3504.719272	489868.273195	41.947495
3504.553028	489844.949557	41.952500
3504.883338	489827.270927	41.957504
3504.533033	489852.651543	41.962509
3504.630955	489842.759185	41.967514
3504.277268	489818.401478	41.972519
3504.213843	489824.692150	41.977524
3504.947517	489806.291291	41.982528
3504.969451	489782.887184	41.987533
3504.503256	489778.908782	41.992538
3504.438313	489817.768081	41.997543
3504.586551	489776.413677	42.002548
3505.040260	489731.313391	42.007552
3504.528582	489750.844151	42.012557
3504.468761	489779.420605	42.017562
3504.670443	489764.294782	42.022567
3503.860668	489732.259480	42.027572
3504.753288	489698.790088	42.032576
3504.419165	489712.265362	42.037581
3504.442047	489727.153077	42.042586
3504.443647	489749.692416	42.047591
3504.550203	489729.871075	42.052596
3504.519792	489699.384017	42.057600
3504.372498	489687.706900	42.062605
3504.675581	489684.164053	42.067610
3504.755839	489686.531937	42.072615
3504.656126	489695.462238	42.077620
3504.629436	489693.389740	42.082624
3504.621442	489673.079935	42.087629
3504.818646	489645.190667	42.092634
3505.049688	489653.055690	42.097639
3504.984743	489648.406029	42.102644
3504.767649	489625.191458	42.107648
3504.611270	489630.433213	42.112653
3504.752403	489593.536829	42.117658
3504.715791	489571.813204	42.122663
3504.797776	489544.448510	42.127668
3505.132873	489574.381096	42.132672
3504.862796	489551.985229	42.137677
3505.232894	489517.534424	42.142682
3504.995459	489504.959715	42.147687
3504.832761	489532.387820	42.152692
3504.787710	489490.658129	42.157696
3505.143653	489444.863491	42.162701
3505.069617	489465.338407	42.167706
3504.954175	489447.020751	42.172711
3504.941835	489420.683819	42.177716
3504.952930	489441.449216	42.182720
3504.589539	489403.416563	42.187725
3504.537010	489381.847190	42.192730
3504.264096	489400.327538	42.197735
3504.574720	489397.340615	42.202740
3504.920279	489380.520238	42.207744
3504.514051	489391.626502	42.212749
3504.587779	489382.446851	42.217754
3504.589511	489348.661781	42.222759
3504.361790	489315.064871	42.227764
3504.782030	489345.896097	42.232768
3504.625770	489325.102832	42.237773
3505.087421	489292.561922	42.242778
3504.703956	489302.600947	42.247783
3504.707320	489268.866129	42.252788
3504.933786	489275.465730	42.257792
3504.567596	489244.828401	42.262797
3505.213758	489226.592769	42.267802
3505.149237	489225.083373	42.272807
3504.354467	489248.508959	42.277812
3504.663472	489215.181607	42.282816
3504.828237	489195.451811	42.287821
3504.355943	489200.085135	42.292826
3504.420101	489177.028170	42.297831
3504.831982	489151.788818	42.302836
3504.903049	489166.821316	42.307840
3504.522095	489171.794777	42.312845
3504.907581	489129.793634	42.317850
3504.825819	489150.624678	42.322855
3504.344191	489121.474313	42.327860
3505.011318	489082.822268	42.332864
3504.752364	489104.745073	42.337869
3504.628256	489102.080077	42.342874
3504.812815	489083.258781	42.347879
3504.746405	489047.407187	42.352884
3505.065658	489055.309170	42.357888
3504.537383	489036.296576	42.362893
3504.913724	489014.456390	42.367898
3504.774470	489029.066363	42.372903
3504.717065	488994.074341	42.377908
3504.663796	489012.722962	42.382912
3504.613673	489007.057746	42.387917
3503.906719	488979.411706	42.392922
3504.747480	488955.775853	42.397927
3504.534756	489005.398595	42.402932
3504.596928	488965.170382	42.407936
3504.374157	488942.361092	42.412941
3504.532771	488962.850434	42.417946
3504.833077	488932.613787	42.422951
3504.528771	488916.047669	42.427956
3504.910040	488932.145692	42.432960
3504.700794	488900.824511	42.437965
3504.955322	488886.348125	42.442970
3504.426004	488909.276295	42.447975
3504.386473	488877.472375	42.452980
3504.769271	488837.649094	42.457984
3504.549483	488876.534800	42.462989
3504.445998	488845.146158	42.467994
3505.066896	488834.917350	42.472999
3504.337155	488860.713839	42.478004
3504.405772	488807.567707	42.483008
3504.725439	488784.571188	42.488013
3504.771913	488824.883865	42.493018
3504.682464	488799.976548	42.498023
3504.557824	488765.957145	42.503028
3505.035866	488780.469745	42.508032
3504.742074	488792.115775	42.513037
3504.312337	488760.018756	42.518042
3504.900189	488716.617071	42.523047
3504.631951	488736.211705	42.528052
3504.488311	488753.051338	42.533056
3504.047042	488718.879280	42.538061
3504.636686	488683.480496	42.543066
3504.707914	488731.691427	42.548071
3504.178621	488720.529970	42.553076
3504.969520	488676.589566	42.558080
3504.371454	488699.630162	42.563085
3504.469930	488700.880911	42.568090
3504.533812	488675.088084	42.573095
3504.373590	488666.603561	42.578100
3504.867106	488634.968254	42.583104
3504.567659	488663.381651	42.588109
3504.637428	488652.632008	42.593114
3504.824030	488616.840918	42.598119
3504.462038	488642.275656	42.603124
3504.289989	488598.740536	42.608128
3504.449208	488591.826415	42.613133
3504.487644	488568.012966	42.618138
3504.542563	488562.736247	42.623143
3504.321199	488586.983790	42.628148
3504.559575	488547.790575	42.633152
3504.605103	488555.482761	42.638157
3504.487939	488583.918121	42.643162
3504.519551	488515.580839	42.648167
3504.464249	488547.400300	42.653172
3504.430378	488541.073874	42.658176
3504.754619	488513.669403	42.663181
3504.478899	488529.466374	42.668186
3504.681937	488499.041794	42.673191
3504.768955	488501.256796	42.678196
3504.919492	488478.489254	42.683200
3504.636670	488484.865701	42.688205
3504.713325	488452.333546	42.693210
3505.000312	488440.384403	42.698215
3504.470667	488473.899896	42.703220
3504.472296	488428.918618	42.708224
3504.897362	488429.104680	42.713229
3504.527088	488450.691254	42.718234
3504.421501	488390.327925	42.723239
3504.366691	488412.573844	42.728244
3504.219517	488400.085443	42.733248
3504.746278	488376.093265	42.738253
3504.684255	488399.809319	42.743258
3504.601407	488378.142287	42.748263
3504.354391	488369.367421	42.753268
3505.151147	488339.253984	42.758272
3504.692136	488370.428385	42.763277
3504.200197	488337.985900	42.768282
3504.838741	488334.440439	42.773287
3504.634932	488312.539177	42.778292
3504.683959	488313.037948	42.783296
3504.094216	488306.444716	42.788301
3504.551962	488282.969876	42.793306
3504.675609	488316.078464	42.798311
3504.222067	488276.538156	42.803316
3504.414618	488251.281620	42.808321
3504.221314	488274.005484	42.813325
3504.532655	488263.622678	42.818330
3504.280242	488268.069510	42.823335
3504.588819	488245.479330	42.828340
3504.341219	488249.570821	42.833345
3504.657139	488239.187279	42.838349
3504.346191	488210.616393	42.843354
3504.690532	488249.870114	42.848359
3504.514719	488206.993203	42.853364
3504.351233	488205.347403	42.858369
3504.513842	488200.864041	42.863373
3504.297621	488194.616974	42.868378
3504.511702	488199.800571	42.873383
3504.626659	488183.015581	42.878388
3504.699905	488148.710521	42.883393
3504.348088	488185.845579	42.888397
3504.468561	488160.701625	42.893402
3504.509044	488174.777297	42.898407
3503.980568	488120.761170	42.903412
3504.375466	488138.276059	42.908417
3504.609330	488117.267844	42.913421
3504.234903	488141.996043	42.918426
3504.701163	488103.728342	42.923431
3504.074716	488125.001186	42.928436
3504.475561	488098.191872	42.933441
3504.335376	488124.301417	42.938445
3504.058188	488091.875226	42.943450
3504.697779	488076.020328	42.948455
3504.234716	488110.184455	42.953460
3504.518993	488084.052062	42.958465
3504.233081	488076.195003	42.963469
3504.324695	488059.464249	42.968474
3504.264606	488075.835379	42.973479
3504.226478	488048.842099	42.978484
3504.308273	488079.779533	42.983489
3504.268645	488059.472999	42.988493
3504.321221	488071.621934	42.993498
3504.455375	488048.451225	42.998503
3504.279903	488015.147685	43.003508
3504.143535	488052.502229	43.008513
3504.354158	488024.456492	43.013517
3504.309438	488059.162456	43.018522
3504.325152	488021.219076	43.023527
3504.555891	488016.927524	43.028532
3504.098779	488036.400764	43.033537
3503.811595	488037.408578	43.038541
3503.613385	488014.594291	43.043546
3504.263497	487992.253763	43.048551
3504.210442	487999.860444	43.053556
3504.032009	488002.573359	43.058561
3504.574561	487981.769483	43.063565
3504.198906	487986.286514	43.068570
3504.531578	488012.321478	43.073575
3504.163646	488017.749079	43.078580
3504.370946	487999.784258	43.083585
3504.010394	488016.101617	43.088589
3504.257851	488017.379520	43.093594
3504.459863	488015.625280	43.098599
3504.545051	488016.827519	43.103604
3504.230913	488010.747834	43.108609
3504.155196	487994.043469	43.113613
3503.669870	487973.655320	43.118618
3504.573774	487964.698363	43.123623
3504.238951	487997.525378	43.128628
3504.149708	487989.333267	43.133633
3504.061042	487970.807330	43.138637
3504.263267	487945.396893	43.143642
3504.352128	487980.132544	43.148647
3503.827536	487968.159410	43.153652
3504.189753	487965.822634	43.158657
3504.348246	487956.223653	43.163661
3504.059482	487974.758546	43.168666
3503.893398	487954.978442	43.173671
3504.293149	487926.041523	43.178676
3504.367330	487946.443996	43.183681
3504.113867	487982.753416	43.188685
3503.877452	487963.592302	43.193690
3504.349700	487933.276236	43.198695
3503.751796	487978.150251	43.203700
3503.974990	487943.669155	43.208705
3503.850919	487977.526664	43.213709
3504.355521	487958.096460	43.218714
3504.571006	487942.865694	43.223719
3504.055374	487997.401882	43.228724
3504.637080	487991.687157	43.233729
3504.427995	487956.970474	43.238733
3503.847108	487939.484759	43.243738
3504.365052	487899.840778	43.248743
3504.200316	487910.808425	43.253748
3504.437534	487955.347878	43.258753
3504.281569	487949.243174	43.263757
3503.869958	487938.873144	43.268762
3504.389654	487922.429201	43.273767
3504.062828	487947.555374	43.278772
3504.339212	487922.031873	43.283777
3504.428279	487886.457448	43.288781
3504.251884	487893.019894	43.293786
3504.287298	487928.017366	43.298791
3504.245447	487904.772989	43.303796
3504.315514	487925.733347	43.308801
3504.290043	487904.158017	43.313805
3504.423613	487893.853764	43.318810
3504.500376	487864.309275	43.323815
3504.019859	487888.345389	43.328820
3504.442485	487860.063280	43.333825
3504.737183	487878.050148	43.338829
3504.480572	487871.201489	43.343834
3503.914788	487852.902814	43.348839
3504.266275	487816.374976	43.353844
3504.454606	487861.834183	43.358849
3504.444994	487874.246352	43.363853
3503.998570	487863.020634	43.368858
3504.487562	487822.469263	43.373863
3504.217628	487847.789199	43.378868
3504.305460	487807.149232	43.383873
3504.367051	487803.745519	43.388877
3504.190550	487831.279574	43.393882
3504.581983	487799.810982	43.398887
3504.525380	487832.341029	43.403892
3504.316725	487799.498260	43.408897
3504.608184	487765.006052	43.413901
3504.373310	487804.048303	43.418906
3504.963601	487751.272672	43.423911
3504.159509	487781.894701	43.428916
3504.539833	487745.818075	43.433921
3504.158349	487757.275972	43.438925
3504.239474	487721.753150	43.443930
3504.291212	487747.782222	43.448935
3503.830920	487755.048115	43.453940
3504.395357	487718.739714	43.458945
3504.237466	487754.021339	43.463949
3504.060762	487757.899106	43.468954
3504.319742	487721.537675	43.473959
3504.169466	487723.840929	43.478964
3504.469978	487703.378943	43.483969
3504.413118	487732.515231	43.488973
3504.152503	487703.986284	43.493978
3504.147066	487742.232555	43.498983
3504.030529	487717.378756	43.503988
3504.510425	487715.833850	43.508993
3504.185898	487716.037084	43.513997
3504.247960	487692.370774	43.519002
3504.642902	487711.709676	43.524007
3504.635364	487677.467191	43.529012
3504.400228	487659.521321	43.534017
3504.572985	487682.542628	43.539021
3504.343680	487694.229792	43.544026
3504.384228	487671.630639	43.549031
3504.509219	487638.380264	43.554036
3504.328923	487683.644876	43.559041
3504.440229	487662.300936	43.564045
3504.420963	487618.080890	43.569050
3504.482661	487642.892775	43.574055
3504.240082	487612.891805	43.579060
3504.618108	487638.312235	43.584065
3504.495399	487617.765078	43.589069
3504.112280	487612.152075	43.594074
3504.706592	487580.397775	43.599079
3504.294685	487624.078123	43.604084
3503.999170	487596.719631	43.609089
3504.344448	487565.815170	43.614093
3504.162694	487620.856888	43.619098
3504.074295	487614.538771	43.624103
3504.236663	487582.042238	43.629108
3505.049344	487542.300276	43.634113
3504.650720	487531.168119	43.639117
3504.539338	487521.206320	43.644122
3504.862962	487512.391524	43.649127
3504.470117	487507.641193	43.654132
3504.536161	487489.292964	43.659137
3504.471735	487490.164285	43.664141
3504.405974	487491.795670	43.669146
3504.716123	487516.011227	43.674151
3504.194049	487514.725982	43.679156
3504.023983	487483.953496	43.684161
3504.283125	487455.544657	43.689165
3504.260179	487460.411320	43.694170
3504.383612	487473.663889	43.699175
3503.768066	487467.074442	43.704180
3504.003856	487466.479922	43.709185
3503.919984	487479.157369	43.714189
3503.872397	487477.847785	43.719194
3505.085631	487452.986097	43.724199
3504.935167	487450.527661	43.729204
3504.727373	487449.800622	43.734209
3504.515115	487425.569455	43.739213
3504.547781	487405.453425	43.744218
3504.818067	487399.889059	43.749223
3504.777745	487396.400067	43.754228
3504.999060	487379.901503	43.759233
3505.080649	487370.162411	43.764237
3504.568980	487350.588271	43.769242
3504.677736	487324.279950	43.774247
3504.480469	487364.988845	43.779252
3504.406674	487382.578508	43.784257
3504.346825	487341.201033	43.789261
3503.885071	487322.936062	43.794266
3504.431792	487305.271544	43.799271
3504.163780	487315.698624	43.804276
3504.282090	487339.235524	43.809281
3504.453189	487347.110980	43.814285
3503.640235	487337.563912	43.819290
3504.483306	487300.957393	43.824295
3504.555653	487328.554157	43.829300
3504.417519	487316.874132	43.834305
3503.937645	487288.227245	43.839309
3504.233389	487257.330115	43.844314
3504.417521	487291.494731	43.849319
3503.844000	487302.577993	43.854324
3504.461977	487268.387882	43.859329
3504.350324	487260.097684	43.864333
3504.011403	487294.091678	43.869338
3503.879385	487292.694110	43.874343
3503.972957	487290.653000	43.879348
3504.289386	487270.036062	43.884353
3503.995273	487260.103007	43.889357
3504.062429	487248.897068	43.894362
3504.336225	487268.914114	43.899367
3503.943788	487255.349262	43.904372
3504.373956	487269.870587	43.909377
3504.549157	487269.640240	43.914381
3504.360511	487250.622831	43.919386
3504.405198	487273.462244	43.924391
3503.960503	487257.727385	43.929396
3504.126107	487222.848829	43.934401
3503.883106	487262.855964	43.939405
3503.570395	487247.049579	43.944410
3504.717691	487216.777657	43.949415
3504.684985	487216.884114	43.954420
3504.498368	487216.862924	43.959425
3504.689508	487245.454183	43.964429
3504.498206	487253.792216	43.969434
3504.640414	487226.617297	43.974439
3504.318512	487198.249253	43.979444
3504.461760	487173.910920	43.984449
3504.354729	487156.096302	43.989453
3504.187636	487195.230400	43.994458
3504.382144	487197.276592	43.999463
3504.030844	487179.399288	44.004468
3503.890154	487170.961667	44.009473
3504.796363	487140.221152	44.014477
3504.398763	487181.772623	44.019482
3504.358082	487181.981656	44.024487
3504.396567	487177.011097	44.029492
3504.335922	487165.217416	44.034497
3504.250732	487148.361835	44.039501
3504.104006	487137.088320	44.044506
3504.486725	487126.389670	44.049511
3504.400545	487136.889424	44.054516
3504.343239	487103.008378	44.059521
3504.574806	487094.309256	44.064525
3504.379547	487119.365066	44.069530
3504.569956	487086.002075	44.074535
3504.182651	487125.829672	44.079540
3504.130125	487073.356399	44.084545
3504.229035	487079.622322	44.089549
3503.868017	487078.362248	44.094554
3504.740316	487045.397992	44.099559
3504.275387	487098.155703	44.104564
3504.409600	487066.068006	44.109569
3504.462617	487080.699742	44.114573
3504.000926	487076.213473	44.119578
3504.507076	487032.364949	44.124583
3504.438372	487051.068589	44.129588
3504.117927	487019.863202	44.134593
3503.967484	487058.994947	44.139597
3503.979329	487048.354870	44.144602
3504.350109	487050.069271	44.149607
3504.479784	487039.359908	44.154612
3503.849514	487034.900273	44.159617
3504.476271	487010.738604	44.164621
3504.330253	487026.769608	44.169626
3504.560481	487014.423281	44.174631
3504.053080	487024.331116	44.179636
3504.252844	486991.928986	44.184641
3504.083414	487033.343401	44.189645
3504.190577	486998.726963	44.194650
3504.131667	487022.140290	44.199655
3504.069813	486983.801841	44.204660
3503.925960	487011.686524	44.209665
3503.902675	486988.691387	44.214669
3503.986751	486951.849555	44.219674
3503.857241	487001.515023	44.224679
3504.254084	486964.370492	44.229684
3504.280436	487000.485578	44.234689
3504.517473	486975.929538	44.239693
3504.041141	486998.041096	44.244698
3504.679334	486956.552462	44.249703
3504.486855	487000.098238	44.254708
3504.345914	486961.772245	44.259713
3504.385863	486975.392963	44.264717
3504.182087	486967.319830	44.269722
3504.391624	486971.187367	44.274727
3504.199677	486960.326160	44.279732
3504.129875	486990.782739	44.284737
3504.261404	486953.933411	44.289741
3504.241312	486992.943373	44.294746
3504.186597	486937.481242	44.299751
3504.043979	486933.856358	44.304756
3504.117829	486922.598512	44.309761
3504.431510	486945.243827	44.314765
3504.227106	486922.986453	44.319770
3504.258672	486939.850654	44.324775
3504.404797	486929.442580	44.329780
3504.469432	486945.389700	44.334785
3504.347215	486909.593557	44.339789
3504.131975	486892.403696	44.344794
3504.282360	486888.783152	44.349799
3504.180601	486921.625838	44.354804
3503.741479	486889.881753	44.359809
3504.343587	486898.651783	44.364813
3504.250212	486928.250995	44.369818
3504.262805	486905.756671	44.374823
3504.573314	486882.759308	44.379828
3504.561496	486891.575715	44.384833
3504.573875	486856.163467	44.389837
3503.951871	486891.520038	44.394842
3504.205888	486867.721051	44.399847
3504.627326	486860.156959	44.404852
3504.086253	486847.932430	44.409857
3504.256436	486849.627895	44.414861
3503.863047	486825.525911	44.419866
3504.044284	486833.805246	44.424871
3503.900878	486826.330415	44.429876
3503.899410	486849.734873	44.434881
3504.123014	486836.072356	44.439885
3504.125282	486826.700135	44.444890
3504.278746	486853.727518	44.449895
3504.489316	486815.041724	44.454900
3504.367288	486850.218032	44.459905
3504.461050	486851.672283	44.464909
3503.983911	486815.729426	44.469914
3504.203277	486793.354265	44.474919
3504.094863	486830.605463	44.479924
3503.494371	486805.624332	44.484929
3504.474295	486765.347739	44.489933
3503.824309	486792.654172	44.494938
3503.916307	486823.895983	44.499943
3504.366119	486796.671836	44.504948
3504.249122	486812.242505	44.509953
3504.044896	486804.220033	44.514957
3504.309860	486820.591522	44.519962
3504.209870	486815.440120	44.524967
3503.910263	486817.615108	44.529972
3504.314198	486823.326319	44.534977
3504.459454	486783.333660	44.539981
3504.233355	486785.750327	44.544986
3504.181919	486791.533520	44.549991
3504.722400	486772.603031	44.554996
3504.245085	486806.923715	44.560001
3504.369295	486767.288959	44.565005
3504.259266	486779.869686	44.570010
3504.375103	486757.966775	44.575015
3504.628389	486734.015762	44.580020
3504.270270	486774.396724	44.585025
3504.179071	486757.187137	44.590029
3504.184348	486743.255108	44.595034
3504.018234	486753.159800	44.600039
3504.429367	486714.543422	44.605044
3504.346709	486739.885884	44.610049
3504.224820	486706.115661	44.615053
3503.748133	486736.333000	44.620058
3504.282686	486704.941305	44.625063
3504.096023	486746.612359	44.630068
3503.840245	486715.801524	44.635073
3504.533384	486703.939081	44.640077
3504.276203	486759.755083	44.645082
3504.338371	486740.342913	44.650087
3504.078054	486701.275384	44.655092
3504.130273	486684.954925	44.660097
3504.406193	486701.122149	44.665101
3504.067230	486713.739103	44.670106
3503.737565	486675.695660	44.675111
3504.495329	486685.099754	44.680116
3504.332712	486713.038496	44.685121
3504.161312	486695.638894	44.690125
3504.621080	486668.463651	44.695130
3504.414775	486690.076954	44.700135
3504.407349	486675.842931	44.705140
3504.420827	486634.351019	44.710145
3504.418462	486674.878600	44.715149
3504.144310	486678.214737	44.720154
3504.823328	486630.994480	44.725159
3504.389042	486650.566838	44.730164
3504.172672	486608.604608	44.735169
3504.503506	486605.259446	44.740173
3504.486650	486641.888629	44.745178
3504.499194	486594.874939	44.750183
3504.238142	486599.171544	44.755188
3504.416512	486596.661025	44.760193
3504.530470	486585.801916	44.765197
3504.409937	486585.922257	44.770202
3504.321961	486595.358748	44.775207
3504.692853	486562.219616	44.780212
3504.220002	486559.508062	44.785217
3504.144627	486558.050829	44.790221
3504.124422	486529.127514	44.795226
3504.111208	486548.886721	44.800231
3504.168262	486566.861727	44.805236
3504.235263	486539.495083	44.810241
3504.507138	486549.178677	44.815245
3504.252560	486512.136228	44.820250
3503.929910	486526.523806	44.825255
3504.194224	486494.059973	44.830260
3503.968286	486541.006264	44.835265
3504.074179	486508.314196	44.840269
3504.394240	486529.489872	44.845274
3504.498816	486509.513513	44.850279
3503.995638	486540.140623	44.855284
3504.150192	486515.698349	44.860289
3504.584816	486532.296567	44.865293
3504.050896	486486.534146	44.870298
3503.874572	486491.729254	44.875303
3504.420184	486489.616613	44.880308
3503.971406	486493.942912	44.885313
3504.294171	486488.319329	44.890317
3504.217764	486492.840071	44.895322
3504.071618	486482.579267	44.900327
3504.202509	486514.170053	44.905332
3503.894067	486508.291623	44.910337
3504.341771	486478.585047	44.915341
3504.040690	486508.217735	44.920346
3504.000663	486488.517506	44.925351
3504.177121	486478.813626	44.930356
3504.015858	486474.431709	44.935361
3504.110451	486488.500072	44.940365
3504.035166	486472.402222	44.945370
3504.238758	486482.755217	44.950375
3504.450033	486478.314420	44.955380
3504.473466	486467.773509	44.960385
3504.700421	486483.087445	44.965389
3504.321148	486447.685682	44.970394
3504.154461	486454.044448	44.975399
3504.416427	486440.274268	44.980404
3504.240577	486436.553222	44.985409
3504.157895	486452.473377	44.990413
3504.260909	486443.692959	44.995418
3503.850256	486449.533030	45.000423
3504.049237	486447.323191	45.005428
3504.018676	486454.268357	45.010433
3504.392258	486441.645707	45.015437
3504.022958	486430.862889	45.020442
3504.307119	486398.598396	45.025447
3504.145391	486430.235569	45.030452
3504.025418	486408.065570	45.035457
3504.411441	486424.519585	45.040461
3504.759993	486408.202714	45.045466
3504.258494	486415.475624	45.050471
3504.200991	486393.245076	45.055476
3504.380158	486379.437279	45.060481
3504.467754	486382.665632	45.065485
3504.220315	486359.401209	45.070490
3504.250990	486385.182165	45.075495
3504.222976	486356.107845	45.080500
3504.295412	486374.739178	45.085505
3504.291793	486386.898066	45.090509
3504.251073	486334.826182	45.095514
3504.035471	486364.850860	45.100519
3504.312723	486356.296163	45.105524
3504.337370	486340.131748	45.110529
3503.944275	486354.682568	45.115533
3504.276699	486335.683213	45.120538
3504.306499	486370.988383	45.125543
3504.632859	486305.686852	45.130548
3504.302058	486322.963488	45.135553
3504.221797	486306.207706	45.140557
3503.909471	486314.413295	45.145562
3504.380705	486295.088001	45.150567
3504.047384	486326.904445	45.155572
3504.150024	486302.926044	45.160577
3504.304817	486306.498409	45.165581
3503.972148	486319.671886	45.170586
3504.305317	486290.084441	45.175591
3503.855919	486308.595675	45.180596
3504.106247	486270.206457	45.185601
3504.066619	486299.088905	45.190605
3503.728704	486282.373824	45.195610
3504.060821	486248.075097	45.200615
3503.960038	486295.204849	45.205620
3504.080625	486259.166475	45.210625
3504.387575	486288.855382	45.215629
3504.476586	486262.194104	45.220634
3503.975211	486291.352183	45.225639
3504.418622	486302.832551	45.230644
3504.125450	486295.887782	45.235649
3504.462488	486258.548697	45.240653
3503.841026	486284.888801	45.245658
3504.159473	486244.816986	45.250663
3504.387723	486273.302512	45.255668
3503.853241	486280.732666	45.260673
3504.425227	486229.830159	45.265677
3504.060086	486262.563620	45.270682
3504.109643	486257.844373	45.275687
3504.424774	486254.957573	45.280692
3504.052694	486262.260747	45.285697
3504.426674	486250.296489	45.290701
3504.224604	486245.313048	45.295706
3504.521781	486214.768633	45.300711
3504.587753	486228.689730	45.305716
3504.612939	486192.159707	45.310721
3504.422298	486232.920619	45.315725
3504.469488	486187.014978	45.320730
3504.151963	486202.465854	45.325735
3504.726647	486151.258750	45.330740
3504.404436	486193.357711	45.335745
3504.143851	486185.597188	45.340749
3503.578564	486188.624801	45.345754
3504.400612	486173.144779	45.350759
3504.685013	486126.644239	45.355764
3504.388339	486133.834221	45.360769
3504.559163	486168.610870	45.365773
3504.479164	486183.618937	45.370778
3504.341465	486141.643251	45.375783
3504.439808	486136.156357	45.380788
3504.023932	486115.856563	45.385793
3504.524382	486098.299571	45.390797
3504.230090	486105.033243	45.395802
3504.622450	486105.579129	45.400807
3504.599794	486108.115707	45.405812
3504.086030	486083.525209	45.410817
3504.142782	486101.956643	45.415821
3504.244430	486063.083907	45.420826
3503.971798	486083.036576	45.425831
3503.953726	486077.365423	45.430836
3504.399401	486052.623244	45.435841
3504.246764	486090.034851	45.440845
3504.097361	486065.792027	45.445850
3504.106311	486078.455730	45.450855
3504.209325	486069.675142	45.455860
3503.964930	486065.762216	45.460865
3504.141806	486073.080018	45.465869
3504.002286	486051.520624	45.470874
3503.966392	486030.603417	45.475879
3503.909953	486051.535163	45.480884
3503.756829	486024.101254	45.485889
3504.297364	486032.830755	45.490893
3503.867794	486057.874323	45.495898
3504.261917	486022.957467	45.500903
3504.361767	486056.175055	45.505908
3503.950945	486050.920593	45.510913
3504.155766	486037.969727	45.515917
3504.105551	486072.173559	45.520922
3504.077963	486033.625152	45.525927
3504.460793	486054.284825	45.530932
3504.282241	486046.460620	45.535937
3504.357066	486062.102900	45.540941
3504.334485	486025.428128	45.545946
3504.223847	485993.529318	45.550951
3504.444648	486036.454692	45.555956
3504.033867	486034.290520	45.560961
3503.710680	486014.178611	45.565965
3504.503809	486004.680991	45.570970
3504.482413	485990.803293	45.575975
3504.190728	485982.237030	45.580980
3503.879528	486010.808207	45.585985
3503.838188	485984.268467	45.590989
3504.137273	485967.857720	45.595994
3504.253006	485971.334999	45.600999
3504.195198	486011.366135	45.606004
3503.868544	486011.012450	45.611009
3504.251210	485988.407899	45.616013
3504.093998	485982.302761	45.621018
3504.472567	485966.538041	45.626023
3504.272428	485968.089472	45.631028
3504.179273	486008.075540	45.636033
3503.780777	485965.228794	45.641037
3504.232774	485923.970003	45.646042
3504.032534	485967.924635	45.651047
3504.116747	485942.226228	45.656052
3503.799486	485928.901856	45.661057
3503.784385	485974.853649	45.666061
3503.781468	485943.697643	45.671066
3503.760298	485938.938835	45.676071
3504.261057	485959.377328	45.681076
3503.804716	485948.050726	45.686081
3504.332533	485913.619150	45.691085
3504.120601	485934.930227	45.696090
3503.986300	485964.740037	45.701095
3504.084678	485928.299265	45.706100
3503.804392	485982.550688	45.711105
3503.704848	485948.978243	45.716109
3504.028564	485929.929203	45.721114
3503.800981	485987.566565	45.726119
3503.978081	485950.404143	45.731124
3503.954829	485987.896821	45.736129
3504.079087	485943.143614	45.741133
3503.936245	485972.650796	45.746138
3503.771042	485978.654858	45.751143
3504.185623	485968.862424	45.756148
3503.952138	485981.209883	45.761153
3504.076880	485960.317871	45.766157
3503.943031	485959.173799	45.771162
3504.428293	485996.788731	45.776167
3504.354660	485991.430298	45.781172
3504.172734	485987.456822	45.786177
3503.811935	485997.848621	45.791181
3504.472747	485970.640617	45.796186
3504.163532	485985.482423	45.801191
3504.127777	485950.481397	45.806196
3504.233510	485933.797215	45.811201
3503.829130	485959.140895	45.816205
3504.136821	485937.257386	45.821210
3504.299524	485952.176614	45.826215
3504.312473	485963.826542	45.831220
3504.120889	485942.325915	45.836225
3504.233440	485940.534967	45.841229
3504.345337	485958.653858	45.846234
3504.104679	485945.925321	45.851239
3504.261090	485912.363019	45.856244
3503.881373	485917.995716	45.861249
3503.977541	485886.165364	45.866253
3504.033257	485935.804315	45.871258
3504.405400	485895.723287	45.876263
3504.281167	485909.016084	45.881268
3503.819230	485928.238919	45.886273
3504.356018	485889.043751	45.891277
3504.130973	485920.134499	45.896282
3503.879240	485950.672144	45.901287
3504.174497	485915.466754	45.906292
3503.979624	485939.308179	45.911297
3504.233826	485951.173290	45.916301
3504.207504	485900.617779	45.921306
3504.248713	485868.188151	45.926311
3504.433250	485875.251513	45.931316
3503.923994	485918.241877	45.936321
3504.208949	485881.619546	45.941325
3504.284328	485877.504057	45.946330
3504.031782	485913.057338	45.951335
3503.780670	485881.484510	45.956340
3504.326608	485863.109537	45.961345
3504.103263	485905.497468	45.966349
3503.896422	485879.996962	45.971354
3503.961547	485875.021855	45.976359
3504.351247	485909.865701	45.981364
3503.961531	485858.759583	45.986369
3504.071440	485860.971275	45.991373
3503.874262	485875.694136	45.996378
3504.114868	485860.863034	46.001383
3504.275391	485857.645984	46.006388
3504.022203	485878.406371	46.011393
3504.257185	485850.657568	46.016397
3504.263526	485885.562048	46.021402
3504.475601	485868.557036	46.026407
3504.209555	485872.854591	46.031412
3503.968401	485876.641600	46.036417
3504.050948	485863.557959	46.041421
3504.410124	485870.239093	46.046426
3504.312841	485849.635358	46.051431
3504.470443	485824.989079	46.056436
3504.278508	485839.964444	46.061441
3504.388838	485840.909542	46.066445
3504.606312	485840.317870	46.071450
3504.016079	485838.891294	46.076455
3504.084548	485804.886753	46.081460
3504.195430	485774.725714	46.086465
3503.937767	485818.031166	46.091469
3504.430930	485815.926744	46.096474
3504.693406	485780.574305	46.101479
3504.474849	485813.184040	46.106484
3504.353784	485812.848518	46.111489
3504.441702	485760.096148	46.116493
3504.522682	485783.438214	46.121498
3504.237190	485757.291379	46.126503
3504.596523	485767.518822	46.131508
3504.597703	485760.426013	46.136513
3504.256648	485747.206599	46.141517
3504.754503	485722.861042	46.146522
3504.326103	485751.805757	46.151527
3504.408561	485716.785621	46.156532
3504.104976	485748.952951	46.161537
3504.613663	485696.843164	46.166541
3504.307188	485720.145222	46.171546
3504.025115	485686.297199	46.176551
3504.742282	485672.707833	46.181556
3504.391674	485718.105327	46.186561
3503.780694	485699.558420	46.191565
3504.478992	485663.478284	46.196570
3504.335785	485686.602592	46.201575
3504.448125	485640.989319	46.206580
3504.044179	485660.000609	46.211585
3504.124641	485653.857802	46.216589
3504.536135	485646.852086	46.221594
3504.152640	485663.884332	46.226599
3504.381898	485634.717597	46.231604
3503.907577	485646.850025	46.236609
3503.966827	485623.029620	46.241613
3504.414221	485590.636649	46.246618
3504.076469	485635.475026	46.251623
3504.304461	485588.678131	46.256628
3504.011539	485629.912442	46.261633
3504.335291	485592.523504	46.266637
3504.432802	485622.347867	46.271642
3503.847784	485614.283757	46.276647
3504.321889	485615.829974	46.281652
3503.981009	485618.112942	46.286657
3504.243965	485595.273541	46.291661
3504.071761	485591.703741	46.296666
3504.298439	485556.356548	46.301671
3504.534860	485603.991979	46.306676
3504.669252	485573.522937	46.311681
3504.514869	485568.177149	46.316685
3504.445760	485594.430895	46.321690
3504.320142	485537.304084	46.326695
3504.395645	485566.422744	46.331700
3504.062415	485559.636025	46.336705
3504.255845	485541.873743	46.341709
3504.145563	485549.794413	46.346714
3504.078388	485551.679495	46.351719
3504.347157	485533.905297	46.356724
3504.257220	485548.206163	46.361729
3504.207440	485497.248005	46.366733
3504.225380	485510.163971	46.371738
3503.972267	485510.001301	46.376743
3503.971931	485503.313934	46.381748
3504.158983	485515.392575	46.386753
3503.911022	485494.812275	46.391757
3504.092352	485511.147440	46.396762
3503.949245	485534.119929	46.401767
3504.333730	485516.327426	46.406772
3503.700468	485529.650276	46.411777
3503.871537	485499.732603	46.416781
3504.146469	485511.088089	46.421786
3503.830107	485521.625106	46.426791
3504.371495	485498.792247	46.431796
3504.088288	485537.289468	46.436801
3503.700432	485512.374366	46.441805
3504.133513	485495.992701	46.446810
3504.031711	485549.710512	46.451815
3503.933052	485539.391036	46.456820
3503.858472	485533.576668	46.461825
3503.747777	485510.593575	46.466829
3504.478858	485498.623074	46.471834
3503.942200	485534.576592	46.476839
3503.971241	485524.996856	46.481844
3504.211826	485488.127480	46.486849
3504.456604	485482.110634	46.491853
3503.987194	485506.350620	46.496858
3504.196852	485484.178119	46.501863
3504.638555	485462.931499	46.506868
3504.280919	485508.887880	46.511873
3504.130858	485524.110183	46.516877
3504.387883	485478.726969	46.521882
3504.350258	485463.584902	46.526887
3504.526212	485491.218596	46.531892
3504.239228	485469.225898	46.536897
3503.797568	485465.293364	46.541901
3504.413151	485441.030169	46.546906
3504.343747	485483.496022	46.551911
3504.455789	485455.360784	46.556916
3504.148479	485432.003376	46.561921
3503.961922	485441.354689	46.566925
3503.971165	485426.458496	46.571930
3503.888415	485407.169210	46.576935
3503.889126	485448.712136	46.581940
3504.015544	485435.367959	46.586945
3504.185467	485416.646694	46.591949
3504.187846	485451.248614	46.596954
3503.792250	485437.429660	46.601959
3504.151995	485400.997244	46.606964
3504.130033	485452.929523	46.611969
3503.942273	485421.852550	46.616973
3504.037766	485447.168559	46.621978
3504.249683	485420.942650	46.626983
3504.174736	485439.648845	46.631988
3504.561054	485408.987740	46.636993
3503.905105	485432.092069	46.641997
3504.144890	485395.171979	46.647002
3504.240670	485401.134971	46.652007
3503.941624	485393.633518	46.657012
3504.355001	485379.990637	46.662017
3504.195491	485415.834105	46.667021
3504.347550	485373.101672	46.672026
3504.022155	485422.548870	46.677031
3504.076955	485388.444430	46.682036
3504.504037	485391.872606	46.687041
3504.331933	485406.439875	46.692045
3504.605271	485344.537839	46.697050
3504.162411	485394.763611	46.702055
3504.339601	485355.573533	46.707060
3504.283964	485380.964178	46.712065
3504.245937	485360.755853	46.717069
3504.570537	485353.611778	46.722074
3504.350453	485342.500788	46.727079
3504.272485	485315.965916	46.732084
3504.186953	485338.726887	46.737089
3504.089547	485308.851351	46.742093
3504.224970	485338.619499	46.747098
3504.284428	485341.599162	46.752103
3504.405084	485329.421061	46.757108
3504.048149	485309.364411	46.762113
3503.973664	485293.316110	46.767117
3504.223544	485308.576697	46.772122
3504.160139	485277.631824	46.777127
3503.897447	485309.641434	46.782132
3503.923585	485272.298913	46.787137
3503.982583	485303.092449	46.792141
3504.336578	485286.723107	46.797146
3504.191551	485293.686783	46.802151
3504.490276	485280.973880	46.807156
3504.122250	485303.576892	46.812161
3504.047372	485291.277683	46.817165
3504.339027	485276.032763	46.822170
3504.239850	485260.190987	46.827175
3504.237827	485255.428983	46.832180
3504.305303	485243.107244	46.837185
3503.963402	485277.206601	46.842189
3504.330887	485229.677510	46.847194
3504.069198	485271.515605	46.852199
3504.283685	485249.595385	46.857204
3504.452668	485257.522699	46.862209
3504.198566	485229.850303	46.867213
3504.300879	485239.156057	46.872218
3504.383792	485214.166163	46.877223
3504.165481	485224.333205	46.882228
3504.177964	485224.077891	46.887233
3504.154587	485204.373715	46.892237
3504.148565	485230.263345	46.897242
3504.124203	485229.709878	46.902247
3504.242500	485233.085560	46.907252
3504.334857	485188.740946	46.912257
3504.004591	485212.148703	46.917261
3504.124068	485174.639252	46.922266
3504.079671	485205.702600	46.927271
3503.917310	485183.436563	46.932276
3504.090586	485198.101390	46.937281
3503.703579	485179.467918	46.942285
3503.754330	485206.361866	46.947290
3503.973681	485189.051127	46.952295
3504.191852	485206.951277	46.957300
3504.344768	485184.990052	46.962305
3503.835778	485210.553901	46.967309
3503.868905	485204.874398	46.972314
3503.748059	485197.901994	46.977319
3504.045763	485198.716184	46.982324
3504.097292	485185.333008	46.987329
3503.674439	485214.075001	46.992333
3504.098635	485183.407550	46.997338
3503.890120	485215.307428	47.002343
3504.187982	485207.052943	47.007348
3504.314335	485193.809935	47.012353
3504.111681	485201.694684	47.017357
3504.124722	485210.051968	47.022362
3504.146321	485188.415478	47.027367
3503.755381	485212.947408	47.032372
3504.123262	485184.366036	47.037377
3503.865978	485205.026468	47.042381
3504.083578	485153.163872	47.047386
3503.832288	485191.859390	47.052391
3503.887124	485174.726630	47.057396
3503.760084	485197.950294	47.062401
3504.002412	485192.491038	47.067405
3504.132126	485221.449663	47.072410
3504.091575	485169.121283	47.077415
3503.941172	485187.383682	47.082420
3504.065770	485176.167456	47.087425
3503.901014	485189.061851	47.092429
3504.286556	485162.098868	47.097434
3503.672194	485186.514154	47.102439
3503.847128	485179.748309	47.107444
3503.957934	485164.835863	47.112449
3503.844643	485177.316827	47.117453
3504.139605	485187.960057	47.122458
3503.861336	485181.772472	47.127463
3504.317312	485158.446082	47.132468
3504.085508	485206.713791	47.137473
3504.004413	485172.934426	47.142477
3504.512964	485181.568047	47.147482
3503.920152	485197.924506	47.152487
3504.106150	485193.943376	47.157492
3504.382530	485199.320595	47.162497
3504.021464	485162.191048	47.167501
3503.780095	485207.927118	47.172506
3503.893267	485186.276153	47.177511
3504.308480	485206.424991	47.182516
3503.835482	485162.321660	47.187521
3503.589241	485182.017775	47.192525
3504.147812	485182.334768	47.197530
3504.399729	485177.481947	47.202535
3504.084841	485202.812476	47.207540
3503.853936	485162.065292	47.212545
3503.774474	485163.648376	47.217549
3503.805572	485138.970552	47.222554
3503.431084	485180.826672	47.227559
3503.738872	485177.079604	47.232564
3503.936144	485214.032305	47.237569
3504.062720	485204.234342	47.242573
3504.410606	485222.975244	47.247578
3503.857947	485187.953203	47.252583
3504.219186	485182.677801	47.257588
3503.822245	485186.033601	47.262593
3503.649671	485160.324073	47.267597
3504.078892	485190.147341	47.272602
3504.007301	485211.335710	47.277607
3503.938108	485166.459286	47.282612
3504.122351	485177.120021	47.287617
3503.832642	485200.876022	47.292621
3504.086843	485164.814482	47.297626
3503.972240	485200.093961	47.302631
3504.006571	485203.938885	47.307636
3503.901001	485176.344263	47.312641
3504.215353	485160.133068	47.317645
3504.050488	485199.676181	47.322650
3503.795225	485176.918192	47.327655
3504.165810	485199.100608	47.332660
3503.894205	485202.993887	47.337665
3503.997691	485192.236973	47.342669
3503.962160	485190.317372	47.347674
3504.071780	485170.896118	47.352679
3504.195582	485206.289894	47.357684
3504.427073	485170.586595	47.362689
3503.781615	485216.893140	47.367693
3504.054511	485187.820157	47.372698
3503.921310	485198.936356	47.377703
3504.047762	485179.867091	47.382708
3504.224303	485211.655454	47.387713
3503.750224	485191.262556	47.392717
3504.451303	485196.370000	47.397722
3504.163655	485185.472250	47.402727
3504.216167	485154.204880	47.407732
3504.164806	485163.028330	47.412737
3504.169122	485153.705632	47.417741
3504.281071	485152.826640	47.422746
3504.317736	485179.621525	47.427751
3504.391878	485153.417028	47.432756
3504.365065	485171.710572	47.437761
3503.969965	485141.375198	47.442765
3504.107868	485159.186752	47.447770
3503.749454	485126.869701	47.452775
3503.970528	485124.605558	47.457780
3504.198262	485146.303982	47.462785
3504.224401	485114.635413	47.467789
3504.467862	485150.972977	47.472794
3503.952007	485118.832785	47.477799
3503.802443	485152.851298	47.482804
3504.440654	485127.722863	47.487809
3503.941330	485144.317907	47.492813
3504.353575	485118.515892	47.497818
3504.125117	485125.138173	47.502823
3504.070925	485140.142974	47.507828
3504.152096	485119.054286	47.512833
3504.186585	485132.119879	47.517837
3504.153214	485078.371553	47.522842
3504.033930	485108.129650	47.527847
3504.163603	485080.396384	47.532852
3504.161461	485106.082915	47.537857
3504.240484	485090.770129	47.542861
3504.186002	485108.105506	47.547866
3504.467098	485082.374835	47.552871
3504.254304	485108.145320	47.557876
3504.437867	485064.343299	47.562881
3504.048786	485072.814861	47.567885
3504.280656	485068.066507	47.572890
3504.031297	485071.044358	47.577895
3504.515849	485046.041430	47.582900
3504.418903	485060.242438	47.587905
3504.364054	485054.171490	47.592909
3504.394469	485065.211242	47.597914
3504.445262	485017.630358	47.602919
3504.120647	485032.475330	47.607924
3504.297730	485007.318294	47.612929
3504.052028	485030.611578	47.617933
3504.714662	485018.296956	47.622938
3504.143383	485032.927597	47.627943
3504.005188	485014.406631	47.632948
3504.345420	484995.556713	47.637953
3504.409647	485002.031450	47.642957
3504.527038	484984.078019	47.647962
3504.197328	484999.075812	47.652967
3504.128209	485005.166317	47.657972
3504.664932	484971.744923	47.662977
3504.203693	484991.171233	47.667981
3504.683750	484942.711703	47.672986
3504.187619	484972.124263	47.677991
3504.171456	484950.949447	47.682996
3504.649145	484938.866660	47.688001
3504.126522	484951.665784	47.693005
3504.090759	484937.485616	47.698010
3504.187949	484927.438840	47.703015
3504.024364	484914.596112	47.708020
3504.197641	484916.645906	47.713025
3503.814812	484928.257687	47.718029
3504.038333	484908.412859	47.723034
3504.343408	484922.651756	47.728039
3504.198744	484918.976149	47.733044
3504.428574	484911.644236	47.738049
3504.403715	484921.932852	47.743053
3504.110772	484911.491756	47.748058
3504.148843	484893.905424	47.753063
3504.213268	484871.704511	47.758068
3504.419929	484891.278676	47.763073
3504.224976	484872.361234	47.768077
3504.335766	484880.804538	47.773082
3504.167954	484890.761119	47.778087
3504.297205	484871.235134	47.783092
3504.273392	484894.442848	47.788097
3504.369429	484855.872547	47.793101
3504.056347	484843.154727	47.798106
3504.387662	484845.382206	47.803111
3504.320222	484840.731767	47.808116
3504.475137	484842.227170	47.813121
3504.231787	484839.884405	47.818125
3504.624131	484845.496714	47.823130
3504.410173	484805.556721	47.828135
3504.113955	484817.104215	47.833140
3504.598264	484777.965752	47.838145
3504.312983	484825.280250	47.843149
3504.205097	484816.329770	47.848154
3504.399196	484773.589367	47.853159
3504.541369	484759.076961	47.858164
3504.498234	484779.400017	47.863169
3504.266460	484775.282176	47.868173
3504.581171	484744.023366	47.873178
3504.255970	484771.737300	47.878183
3504.106290	484746.023602	47.883188
3504.293000	484731.504137	47.888193
3503.968374	484709.161871	47.893197
3503.798897	484743.082925	47.898202
3503.978276	484706.880364	47.903207
3503.982350	484730.083868	47.908212
3503.833988	484750.930226	47.913217
3503.833542	484724.230296	47.918221
3503.986695	484730.285756	47.923226
3504.062340	484744.054405	47.928231
3503.356461	484719.847175	47.933236
3504.052296	484717.761268	47.938241
3503.832607	484726.864842	47.943245
3504.279212	484720.258556	47.948250
3504.064290	484721.508437	47.953255
3504.054141	484740.407724	47.958260
3504.203389	484714.545410	47.963265
3503.892054	484767.285232	47.968269
3504.292390	484736.823501	47.973274
3504.344226	484738.740516	47.978279
3503.631356	484749.087302	47.983284
3504.279035	484719.701061	47.988289
3503.741435	484753.933598	47.993293
3504.102827	484729.507032	47.998298
3503.833299	484758.630780	48.003303
3504.391550	484724.749581	48.008308
3504.195150	484758.472206	48.013313
3504.034592	484729.061730	48.018317
3503.970864	484748.425456	48.023322
3504.087628	484710.611549	48.028327
3504.230601	484731.462546	48.033332
3504.025531	484674.903045	48.038337
3504.186376	484728.581628	48.043341
3504.063289	484713.655136	48.048346
3504.435682	484685.173643	48.053351
3504.198928	484705.628706	48.058356
3504.300541	484733.021916	48.063361
3504.177975	484728.025514	48.068365
3504.237360	484680.037127	48.073370
3504.342804	484671.356848	48.078375
3503.929871	484701.465969	48.083380
3504.052319	484673.327947	48.088385
3504.234246	484660.379777	48.093389
3504.200971	484685.311823	48.098394
3504.151539	484665.357894	48.103399
3504.338311	484670.293445	48.108404
3504.459976	484678.025820	48.113409
3504.025814	484678.499726	48.118413
3504.102893	484661.717645	48.123418
3504.115837	484663.286165	48.128423
3504.396349	484637.808317	48.133428
3504.033117	484625.402265	48.138433
3504.173497	484626.849318	48.143437
3504.337275	484626.266097	48.148442
3504.398773	484626.155021	48.153447
3504.269222	484636.156350	48.158452
3504.281252	484642.892779	48.163457
3504.280632	484600.689413	48.168461
3504.345905	484614.409129	48.173466
3504.093996	484612.422340	48.178471
3504.174700	484573.752570	48.183476
3504.224240	484610.679110	48.188481
3504.500421	484574.106351	48.193485
3504.334719	484579.604280	48.198490
3504.037196	484617.092307	48.203495
3504.440388	484560.233676	48.208500
3504.482637	484578.567530	48.213505
3503.899128	484555.607365	48.218509
3504.261582	484550.382265	48.223514
3504.145350	484584.345845	48.228519
3504.026309	484563.288194	48.233524
3504.431819	484534.446593	48.238529
3503.913731	484586.408951	48.243533
3503.786196	484542.908241	48.248538
3504.534250	484556.925400	48.253543
3504.341119	484541.553865	48.258548
3504.250210	484534.627155	48.263553
3503.933436	484543.898152	48.268557
3504.265440	484496.524863	48.273562
3503.899763	484542.687470	48.278567
3504.000545	484522.152341	48.283572
3504.245408	484521.049655	48.288577
3503.784198	484548.633410	48.293581
3504.172577	484507.280321	48.298586
3503.947952	484542.781047	48.303591
3503.491803	484523.600558	48.308596
3504.520920	484489.492533	48.313601
3503.984922	484533.908815	48.318605
3503.731034	484537.444774	48.323610
3504.042714	484505.730077	48.328615
3503.970260	484531.377820	48.333620
3503.724965	484540.181540	48.338625
3504.193677	484522.780130	48.343629
3503.731516	484545.500233	48.348634
3503.780567	484507.493974	48.353639
3503.785193	484547.518279	48.358644
3504.071462	484523.407313	48.363649
3503.520466	484537.579139	48.368653
3503.842006	484540.112187	48.373658
3503.929807	484558.793512	48.378663
3503.319705	484531.987016	48.383668
3503.699184	484505.378729	48.388673
3503.817352	484560.027154	48.393677
3503.668623	484551.792310	48.398682
3504.682730	484544.842947	48.403687
3503.858326	484560.223254	48.408692
3504.677502	484540.891880	48.413697
3504.443326	484520.865672	48.418701
3504.492832	484557.842983	48.423706
3503.742790	484541.900830	48.428711
3504.052239	484528.071118	48.433716
3504.349885	484513.837944	48.438721
3503.930484	484564.467481	48.443725
3503.635239	484532.291443	48.448730
3504.430639	484506.732043	48.453735
3503.792529	484521.728284	48.458740
3504.235362	484523.988840	48.463745
3504.162303	484481.188687	48.468749
3503.793269	484519.194853	48.473754
3504.143240	484494.415143	48.478759
3504.012996	484519.970705	48.483764
3504.183366	484478.500017	48.488769
3504.264849	484523.781358	48.493773
3504.078790	484504.000851	48.498778
3504.429163	484502.577500	48.503783
3503.832383	484521.164402	48.508788
3504.478641	484470.600172	48.513793
3504.064480	484528.423373	48.518797
3503.506996	484517.111911	48.523802
3503.895603	484489.286208	48.528807
3503.833635	484533.728898	48.533812
3504.076807	484500.505082	48.538817
3503.899405	484522.470900	48.543821
3503.730034	484512.719362	48.548826
3504.376835	484505.473386	48.553831
3503.936783	484540.096201	48.558836
3504.005812	484520.376722	48.563841
3504.247408	484514.765397	48.568845
3503.900234	484529.107673	48.573850
3503.921021	484477.173042	48.578855
3503.734469	484496.607097	48.583860
3504.227457	484478.999152	48.588865
3503.861139	484516.042264	48.593869
3504.094115	484467.367273	48.598874
3504.076420	484499.592825	48.603879
3503.932453	484479.096333	48.608884
3503.879445	484481.587258	48.613889
3504.051288	484484.549291	48.618893
3503.977547	484500.165655	48.623898
3504.043756	484488.502277	48.628903
3503.923196	484504.430026	48.633908
3504.032801	484478.725657	48.638913
3503.957411	484500.624711	48.643917
3504.160397	484500.541937	48.648922
3504.532285	484479.761255	48.653927
3503.933689	484504.884214	48.658932
3504.346888	484471.329486	48.663937
3504.416774	484502.021248	48.668941
3504.357307	484474.570331	48.673946
3504.219829	484485.231632	48.678951
3504.254456	484478.538384	48.683956
3504.465857	484446.788776	48.688961
3504.163271	484478.704736	48.693965
3504.338038	484466.517540	48.698970
3503.942904	484448.847277	48.703975
3503.876078	484480.472648	48.708980
3503.993554	484461.758748	48.713985
3503.994869	484460.137239	48.718989
3504.024590	484481.057071	48.723994
3504.504989	484446.579714	48.728999
3504.071727	484446.952154	48.734004
3504.416857	484432.660751	48.739009
3504.041347	484423.093743	48.744013
3504.163737	484439.185807	48.749018
3504.653123	484406.226904	48.754023
3503.969475	484421.483744	48.759028
3504.104991	484435.344480	48.764033
3504.160189	484420.186924	48.769037
3504.133460	484426.372240	48.774042
3503.904107	484396.516148	48.779047
3503.849870	484404.023108	48.784052
3504.009029	484382.059986	48.789057
3503.950146	484389.669016	48.794061
3504.138623	484392.020454	48.799066
3504.339914	484385.047508	48.804071
3504.119634	484396.937905	48.809076
3503.989622	484399.441010	48.814081
3504.272367	484402.740182	48.819085
3504.252466	484390.381046	48.824090
3504.162680	484386.797994	48.829095
3504.422269	484400.588480	48.834100
3504.706009	484387.877361	48.839105
3504.260848	484374.116142	48.844109
3504.207541	484364.447515	48.849114
3504.204300	484342.611345	48.854119
3503.984059	484364.533447	48.859124
3503.831008	484359.693764	48.864129
3503.982818	484352.019314	48.869133
3503.939933	484359.980484	48.874138
3504.081740	484357.374125	48.879143
3503.798902	484371.351693	48.884148
3504.349012	484360.523727	48.889153
3504.141308	484370.385550	48.894157
3504.035250	484362.447871	48.899162
3504.425776	484368.921913	48.904167
3504.129880	484366.739391	48.909172
3504.176775	484320.018712	48.914177
3503.946075	484342.651805	48.919181
3504.286201	484302.521868	48.924186
3504.121545	484350.578439	48.929191
3503.857063	484332.330104	48.934196
3504.199124	484325.841539	48.939201
3503.433346	484341.314083	48.944205
3504.097575	484334.774601	48.949210
3504.086514	484334.877653	48.954215
3504.020032	484321.208540	48.959220
3504.108917	484333.202108	48.964225
3504.177574	484339.271045	48.969229
3503.995956	484315.284437	48.974234
3504.243201	484349.038986	48.979239
3504.147000	484341.302401	48.984244
3504.544031	484301.974112	48.989249
3504.073236	484333.359579	48.994253
3504.121128	484287.651968	48.999258
3504.302594	484308.193346	49.004263
3504.172757	484283.945189	49.009268
3504.223387	484305.976541	49.014273
3504.171451	484288.555880	49.019277
3504.123873	484301.736337	49.024282
3504.413806	484306.757007	49.029287
3504.139640	484303.811064	49.034292
3504.416752	484250.062029	49.039297
3504.474857	484243.111663	49.044301
3504.158334	484269.659639	49.049306
3504.169692	484249.037024	49.054311
3504.488424	484261.500961	49.059316
3504.498940	484261.701933	49.064321
3503.957995	484230.374872	49.069325
3504.635091	484202.452497	49.074330
3504.480526	484232.065520	49.079335
3503.709924	484222.054204	49.084340
3504.175840	484192.493232	49.089345
3504.243490	484242.337313	49.094349
3504.077893	484246.416689	49.099354
3503.924476	484223.844140	49.104359
3504.351793	484196.011899	49.109364
3504.076792	484235.321061	49.114369
3504.019388	484243.841892	49.119373
3504.032496	484228.133520	49.124378
3504.395848	484205.783267	49.129383
3503.602332	484209.049916	49.134388
3504.109803	484168.234601	49.139393
3504.422684	484165.601178	49.144397
3503.882619	484199.784416	49.149402
3503.948038	484161.572229	49.154407
3503.942309	484189.540495	49.159412
3504.117670	484214.288176	49.164417
3503.895608	484203.024846	49.169421
3504.090518	484167.882800	49.174426
3504.381085	484201.580093	49.179431
3504.017378	484181.067351	49.184436
3504.453044	484203.645950	49.189441
3504.204992	484180.682985	49.194445
3504.185928	484208.045345	49.199450
3504.017116	484177.267367	49.204455
3503.758005	484126.288014	49.209460
3504.250731	484171.505181	49.214465
3504.072930	484146.149790	49.219469
3504.228232	484157.778309	49.224474
3504.396564	484166.060834	49.229479
3504.138554	484137.374179	49.234484
3504.137864	484155.816552	49.239489
3503.794542	484174.414391	49.244493
3503.911436	484131.988768	49.249498
3503.795654	484177.251432	49.254503
3503.671651	484168.759189	49.259508
3504.272754	484135.528842	49.264513
3503.952190	484172.616044	49.269517
3504.210711	484145.773054	49.274522
3504.190914	484161.634493	49.279527
3504.112276	484154.401714	49.284532
3503.809208	484145.431106	49.289537
3503.782867	484167.424116	49.294541
3503.752456	484145.136028	49.299546
3503.965225	484164.912626	49.304551
3504.061050	484148.735125	49.309556
3504.128883	484169.294610	49.314561
3504.199523	484157.225008	49.319565
3503.901277	484173.738434	49.324570
3504.446195	484126.634583	49.329575
3503.862819	484157.075481	49.334580
3503.922048	484099.864539	49.339585
3504.148432	484127.390883	49.344589
3503.668511	484130.354652	49.349594
3504.024573	484095.085672	49.354599
3503.983268	484139.120675	49.359604
3503.789240	484105.559958	49.364609
3503.805319	484134.538171	49.369613
3503.603696	484143.385834	49.374618
3504.470399	484125.819834	49.379623
3504.124936	484141.986090	49.384628
3504.155192	484126.781581	49.389633
3503.773593	484122.028626	49.394637
3503.908122	484125.401937	49.399642
3503.788259	484124.508872	49.404647
3503.746369	484110.785059	49.409652
3504.076730	484137.788297	49.414657
3504.202472	484122.315364	49.419661
3503.520786	484139.649408	49.424666
3504.105675	484111.437481	49.429671
3503.718250	484123.709123	49.434676
3503.843080	484130.427902	49.439681
3503.543773	484157.378636	49.444685
3504.111660	484136.009287	49.449690
3504.274909	484169.017441	49.454695
3504.135773	484136.157419	49.459700
3504.169927	484144.055835	49.464705
3503.902142	484133.965001	49.469709
3504.241251	484111.770469	49.474714
3504.603080	484144.696612	49.479719
3504.383785	484120.411723	49.484724
3504.735684	484138.747718	49.489729
3504.389619	484102.221751	49.494733
3504.319405	484113.125955	49.499738
3504.310202	484080.143970	49.504743
3504.024959	484120.468300	49.509748
3504.179682	484112.793296	49.514753
3504.042040	484075.778346	49.519757
3504.091032	484111.641942	49.524762
3504.218045	484123.882941	49.529767
3504.222120	484087.808264	49.534772
3503.889149	484114.055057	49.539777
3503.709054	484075.780174	49.544781
3504.001447	484052.478309	49.549786
3504.156149	484087.717250	49.554791
3504.014167	484054.756209	49.559796
3504.021527	484087.485144	49.564801
3504.127289	484060.666181	49.569805
3503.746242	484078.408755	49.574810
3503.874584	484050.167566	49.579815
3503.925198	484101.230684	49.584820
3504.100375	484073.286120	49.589825
3504.017922	484078.771033	49.594829
3503.464012	484081.594506	49.599834
3503.768815	484079.215677	49.604839
3503.730461	484080.944349	49.609844
3503.724565	484109.166087	49.614849
3504.034895	484107.242379	49.619853
3503.533346	484110.817558	49.624858
3504.428474	484120.809197	49.629863
3504.263354	484103.355592	49.634868
3503.772886	484103.382419	49.639873
3504.321558	484059.419088	49.644877
3503.842313	484094.150224	49.649882
3503.915136	484063.637869	49.654887
3503.641193	484093.776631	49.659892
3503.929099	484096.821711	49.664897
3503.960225	484074.625147	49.669901
3504.135486	484075.560070	49.674906
3504.027558	484087.483565	49.679911
3503.932130	484088.663934	49.684916
3503.917020	484072.199908	49.689921
3503.814765	484103.274169	49.694925
3504.089985	484088.334908	49.699930
3504.171527	484100.735106	49.704935
3504.110556	484081.238391	49.709940
3504.113909	484100.490830	49.714945
3504.193048	484091.307791	49.719949
3503.955370	484085.417432	49.724954
3504.456848	484080.170234	49.729959
3504.204425	484095.359173	49.734964
3504.499123	484075.502243	49.739969
3504.291224	484066.111230	49.744973
3504.291962	484062.209816	49.749978
3504.211448	484053.406654	49.754983
3503.984445	484064.133002	49.759988
3503.958231	484053.142626	49.764993
3504.183396	484052.245691	49.769997
3504.166756	484052.602955	49.775002
3504.176188	484059.491995	49.780007
3503.996727	484044.219236	49.785012
3504.241935	484044.484449	49.790017
3504.519117	484054.320460	49.795021
3503.900999	484035.874409	49.800026
3504.288381	484023.146671	49.805031
3503.943057	484013.878685	49.810036
3504.243971	484015.503075	49.815041
3504.508387	484029.546392	49.820045
3504.320924	484006.218982	49.825050
3504.447294	484027.630688	49.830055
3504.482894	484006.851986	49.835060
3503.769929	483980.770306	49.840065
3504.004713	483987.370424	49.845069
3503.889442	483975.735421	49.850074
3504.155025	483989.271923	49.855079
3504.104362	483992.623861	49.860084
3504.226229	483981.762039	49.865089
3504.443807	483961.461187	49.870093
3504.231581	483980.697151	49.875098
3504.310015	483973.844807	49.880103
3504.132669	484005.184424	49.885108
3504.563226	483962.354194	49.890113
3504.372155	483984.221448	49.895117
3504.196585	483970.619996	49.900122
3504.540863	483939.963211	49.905127
3504.245442	483975.526830	49.910132
3504.269163	483928.606208	49.915137
3503.970225	483977.698250	49.920141
3503.812057	483939.622296	49.925146
3503.964694	483951.504692	49.930151
3503.745815	483956.859203	49.935156
3504.149799	483919.606351	49.940161
3503.843640	483967.027576	49.945165
3503.746866	483950.069693	49.950170
3504.031082	483962.488612	49.955175
3503.989204	483956.313937	49.960180
3503.807837	483938.254759	49.965185
3504.164143	483975.134025	49.970189
3503.574514	483974.061870	49.975194
3503.952001	483951.101096	49.980199
3503.825025	483986.840736	49.985204
3503.667179	483970.348518	49.990209
3504.452305	483944.587340	49.995213
3503.942083	484011.749834	50.000218
3504.029792	483957.421932	50.005223
3503.954079	483993.052126	50.010228
3503.985382	483961.127524	50.015233
3504.154699	483938.908964	50.020237
3504.129387	483956.190095	50.025242
3504.458480	483931.514300	50.030247
3503.906213	483947.612070	50.035252
3504.231428	483904.849029	50.040257
3504.001524	483928.799800	50.045261
3503.639319	483942.587556	50.050266
3504.143157	483914.844150	50.055271
3504.528228	483906.879327	50.060276
3504.057542	483952.603937	50.065281
3504.311901	483920.086686	50.070285
3504.223206	483942.596467	50.075290
3504.625429	483887.205337	50.080295
3504.380492	483921.950413	50.085300
3503.933197	483880.525404	50.090305
3504.029913	483885.070060	50.095309
3503.832940	483909.572980	50.100314
3504.320832	483886.442682	50.105319
3503.958802	483879.153258	50.110324
3504.273911	483900.889937	50.115329
3503.929862	483899.778963	50.120333
3504.210267	483888.334702	50.125338
3504.197325	483882.459427	50.130343
3504.218555	483909.309177	50.135348
3504.248411	483865.072743	50.140353
3504.542630	483849.724964	50.145357
3503.637947	483870.083810	50.150362
3504.485649	483824.552695	50.155367
3504.378094	483863.025482	50.160372
3503.820471	483865.798906	50.165377
3504.009433	483844.083796	50.170381
3504.196300	483844.459566	50.175386
3504.574636	483816.431857	50.180391
3504.084129	483806.426721	50.185396
3503.784097	483830.692696	50.190401
3504.115393	483798.264413	50.195405
3504.537735	483781.123002	50.200410
3504.513080	483789.841523	50.205415
3504.164791	483792.632537	50.210420
3504.310790	483843.579924	50.215425
3504.415333	483817.976812	50.220429
3504.179661	483797.696761	50.225434
3504.532991	483757.107612	50.230439
3503.919514	483804.780471	50.235444
3504.247901	483788.109914	50.240449
3504.701568	483751.254221	50.245453
3504.007024	483798.787908	50.250458
3503.955429	483772.652083	50.255463
3504.424963	483759.049855	50.260468
3503.929669	483781.522754	50.265473
3503.554832	483752.651329	50.270477
3504.007147	483745.587812	50.275482
3504.198697	483785.533478	50.280487
3503.636368	483763.278356	50.285492
3504.072508	483747.300067	50.290497
3503.950111	483753.399385	50.295501
3503.612380	483784.967373	50.300506
3503.755968	483805.515270	50.305511
3503.764983	483806.729815	50.310516
3503.657629	483798.234778	50.315521
3503.951189	483780.100389	50.320525
3503.513753	483791.214813	50.325530
3504.107964	483786.712878	50.330535
3503.726463	483800.098452	50.335540
3503.635719	483764.544825	50.340545
3503.877510	483795.210536	50.345549
3503.836638	483780.574330	50.350554
3503.868588	483784.875913	50.355559
3503.660044	483791.596833	50.360564
3503.672798	483789.669461	50.365569
3503.892860	483785.783993	50.370573
3503.607251	483814.050368	50.375578
3504.364690	483787.989361	50.380583
3503.922922	483828.997700	50.385588
3503.927685	483785.575714	50.390593
3503.837529	483806.515220	50.395597
3503.995930	483776.242221	50.400602
3504.405407	483810.124067	50.405607
3503.894248	483785.378224	50.410612
3503.702864	483805.827064	50.415617
3503.759562	483778.306135	50.420621
3503.620209	483810.096061	50.425626
3504.135940	483792.078568	50.430631
3503.744921	483838.804186	50.435636
3503.847461	483814.974713	50.440641
3504.138444	483813.358033	50.445645
3503.901501	483841.667343	50.450650
3504.071551	483789.960613	50.455655
3504.041734	483793.258625	50.460660
3503.834669	483800.891307	50.465665
3504.034748	483798.275663	50.470669
3503.912318	483804.425637	50.475674
3504.248310	483800.825848	50.480679
3504.215478	483798.601683	50.485684
3503.744660	483803.540057	50.490689
3504.114650	483811.486861	50.495693
3504.038962	483785.912194	50.500698
3503.933931	483821.192670	50.505703
3503.656122	483799.804618	50.510708
3503.611541	483819.166245	50.515713
3503.461498	483828.056565	50.520717
3503.770549	483819.242392	50.525722
3504.350767	483794.324065	50.530727
3503.686511	483823.714270	50.535732
3503.942633	483809.335144	50.540737
3504.348088	483752.828457	50.545741
3504.213090	483687.844333	50.550746
3504.080191	483663.190549	50.555751
3503.970114	483617.202325	50.560756
3503.812812	483515.386196	50.565761
3503.624323	483420.465248	50.570765
3503.152817	483387.352485	50.575770
3503.478893	483235.449495	50.580775
3503.096931	483143.597855	50.585780
3503.055678	483018.554715	50.590785
3502.648644	482915.508206	50.595789
3502.468288	482750.254231	50.600794
3502.327417	482639.310457	50.605799
3501.853610	482455.200614	50.610804
3502.060517	482341.970703	50.615809
3501.662187	482162.051807	50.620813
3501.625073	481979.033891	50.625818
3500.927407	481801.793902	50.630823
3501.217163	481597.083921	50.635828
3500.487516	481438.037030	50.640833
3500.413492	481194.919769	50.645837
3499.930906	481041.151312	50.650842
3499.598286	480812.765566	50.655847
3499.049892	480581.522810	50.660852
3498.750199	480378.920325	50.665857
3498.424948	480139.377032	50.670861
3497.768792	479916.302355	50.675866
3497.695125	479660.040899	50.680871
3497.377898	479440.505378	50.685876
3496.904129	479193.321775	50.690881
3496.304487	478924.362990	50.695885
3496.265075	478674.215573	50.700890
3495.325361	478407.888229	50.705895
3495.034905	478161.676453	50.710900
3494.723481	477881.660258	50.715905
3494.317547	477597.296390	50.720909
3493.727736	477330.493925	50.725914
3493.183960	477053.847972	50.730919
3492.831605	476767.132411	50.735924
3492.409012	476477.129323	50.740929
3491.673504	476185.194765	50.745933
3491.168840	475908.577578	50.750938
3490.713542	475600.674641	50.755943
3490.029718	475296.655448	50.760948
3489.724753	475000.580676	50.765953
3489.244848	474678.271938	50.770957
3488.388911	474395.454777	50.775962
3488.194665	474069.086690	50.780967
3487.633625	473746.776035	50.785972
3487.148811	473447.057274	50.790977
3486.318804	473114.894062	50.795981
3485.938241	472791.525963	50.800986
3485.363786	472476.953700	50.805991
3484.412706	472153.615044	50.810996
3483.822363	471816.475443	50.816001
3483.679653	471498.423305	50.821005
3482.712633	471161.433946	50.826010
3482.324011	470825.716559	50.831015
3481.740958	470483.230655	50.836020
3480.897396	470181.138222	50.841025
3480.922238	469819.177554	50.846029
3480.067550	469484.779738	50.851034
3479.453753	469146.028703	50.856039
3478.603950	468810.554560	50.861044
3478.013096	468451.557681	50.866049
3477.887132	468100.594133	50.871053
3477.279255	467762.986075	50.876058
3476.374544	467407.976129	50.881063
3475.733745	467055.961006	50.886068
3475.082915	466700.239835	50.891073
3474.360675	466356.897252	50.896077
3473.460812	466012.867241	50.901082
3473.261019	465652.746807	50.906087
3472.299228	465325.653211	50.911092
3471.203806	464935.640394	50.916097
3470.661529	464623.531641	50.921101
3470.318093	464257.273990	50.926106
3469.176115	463900.011609	50.931111
3468.985221	463561.104571	50.936116
3468.337930	463204.513212	50.941121
3467.772242	462855.409390	50.946125
3467.119372	462504.132794	50.951130
3466.497819	462121.804884	50.956135
3465.928066	461784.552968	50.961140
3464.920204	461426.518468	50.966145
3464.628893	461056.343578	50.971149
3463.605069	460699.821363	50.976154
3462.937103	460354.447143	50.981159
3462.312127	459993.741738	50.986164
3461.548974	459628.081124	50.991169
3461.046638	459294.635379	50.996173
3460.266097	458915.624592	51.001178
3459.222731	458590.674511	51.006183
3458.805630	458210.681098	51.011188
3457.865340	457872.666818	51.016193
3457.574745	457507.758896	51.021197
3456.494249	457160.320051	51.026202
3456.100832	456808.759339	51.031207
3455.487401	456438.202963	51.036212
3454.783954	456106.973499	51.041217
3454.297704	455724.006159	51.046221
3453.470873	455396.945995	51.051226
3453.008967	455010.512672	51.056231
3451.786091	454692.941881	51.061236
3451.498079	454297.691385	51.066241
3450.918949	453974.173899	51.071245
3449.964219	453612.149209	51.076250
3449.300612	453237.641372	51.081255
3448.524066	452908.203347	51.086260
3447.828276	452545.917858	51.091265
3446.937486	452189.797331	51.096269
3446.214939	451847.903588	51.101274
3445.402549	451483.945256	51.106279
3444.919214	451150.223908	51.111284
3444.137748	450809.389733	51.116289
3443.718968	450454.131968	51.121293
3442.643549	450116.886334	51.126298
3442.194007	449755.939072	51.131303
3441.169003	449425.526429	51.136308
3440.691317	449065.638660	51.141313
3439.879396	448715.542242	51.146317
3439.095355	448404.514419	51.151322
3438.632188	448047.856793	51.156327
3437.882549	447700.475994	51.161332
3436.857289	447363.588802	51.166337
3436.565609	447008.664718	51.171341
3435.937980	446680.637629	51.176346
3435.073955	446332.036713	51.181351
3434.596689	446013.163357	51.186356
3434.073169	445649.677855	51.191361
3433.421686	445297.322957	51.196365
3431.979736	444957.878923	51.201370
3431.848733	444617.918283	51.206375
3431.128710	444276.167843	51.211380
3429.887140	443941.956785	51.216385
3429.675256	443594.735749	51.221389
3428.908498	443269.628091	51.226394
3428.205866	442934.962578	51.231399
3427.255730	442593.427779	51.236404
3426.849445	442258.452284	51.241409
3426.017078	441927.549952	51.246413
3425.182237	441583.393778	51.251418
3424.756831	441257.240745	51.256423
3423.878622	440933.439460	51.261428
3423.245117	440601.853200	51.266433
3422.535709	440268.700664	51.271437
3422.313894	439941.609564	51.276442
3421.247540	439591.623720	51.281447
3420.567788	439272.795442	51.286452
3419.846181	438940.515435	51.291457
3419.446434	438596.324969	51.296461
3418.823924	438265.771910	51.301466
3417.907458	437922.516969	51.306471
3417.197330	437579.808596	51.311476
3415.850667	437270.250180	51.316481
3415.517706	436942.731119	51.321485
3414.942447	436616.870922	51.326490
3414.256264	436283.915396	51.331495
3413.574876	435951.894100	51.336500
3412.456313	435626.970252	51.341505
3412.144341	435320.601068	51.346509
3411.195705	434998.460506	51.351514
3410.549201	434670.326922	51.356519
3410.454987	434340.883090	51.361524
3409.156884	434020.892826	51.366529
3408.942737	433698.010400	51.371533
3408.051814	433371.016018	51.376538
3407.362571	433050.968206	51.381543
3406.538982	432722.152171	51.386548
3405.935292	432426.230508	51.391553
3405.419338	432070.467531	51.396557
3404.110279	431765.914924	51.401562
3403.565545	431450.623704	51.406567
3403.233987	431129.886228	51.411572
3402.276757	430814.601761	51.416577
3401.804398	430490.475988	51.421581
3400.986451	430188.468312	51.426586
3400.117157	429867.876605	51.431591
3399.998848	429556.710670	51.436596
3399.110933	429227.175195	51.441601
3398.625253	428905.622338	51.446605
3397.751760	428592.685219	51.451610
3396.975170	428276.580003	51.456615
3396.468518	427951.539685	51.461620
3395.541254	427633.165007	51.466625
3394.880940	427333.690357	51.471629
3393.814657	426995.393579	51.476634
3393.582344	426724.060648	51.481639
3392.674429	426379.559522	51.486644
3392.214920	426090.858706	51.491649
3391.743660	425762.636966	51.496653
3390.866133	425445.828651	51.501658
3390.032734	425133.987843	51.506663
3389.267450	424836.127625	51.511668
3388.660100	424503.721342	51.516673
3387.784805	424209.402204	51.521677
3387.317104	423901.655054	51.526682
3386.589971	423585.080764	51.531687
3386.039435	423283.791468	51.536692
3385.212745	422956.811452	51.541697
3384.714919	422670.163429	51.546701
3383.778479	422351.372775	51.551706
3383.160580	422040.047004	51.556711
3382.453439	421732.288138	51.561716
3381.723459	421442.133264	51.566721
3381.097064	421134.253422	51.571725
3380.248372	420827.446854	51.576730
3379.439044	420519.589177	51.581735
3379.246115	420215.746015	51.586740
3378.213642	419914.039205	51.591745
3377.835739	419602.597582	51.596749
3377.118756	419317.372472	51.601754
3376.326734	418990.264390	51.606759
3375.535525	418714.215967	51.611764
3375.099189	418396.215917	51.616769
3374.590253	418074.209763	51.621773
3373.559033	417798.393665	51.626778
3373.005981	417468.918443	51.631783
3372.428205	417181.947771	51.636788
3371.526306	416880.289801	51.641793
3371.034451	416563.929620	51.646797
3370.180960	416253.822443	51.651802
3369.395891	415965.398849	51.656807
3368.806951	415670.183004	51.661812
3368.165171	415362.446530	51.666817
3367.427648	415056.805397	51.671821
3366.792728	414785.928674	51.676826
3366.422904	414464.851256	51.681831
3365.398179	414161.685400	51.686836
3364.847394	413872.314785	51.691841
3364.188781	413572.489773	51.696845
3363.463726	413269.419806	51.701850
3362.472806	412979.322338	51.706855
3362.051947	412682.067915	51.711860
3361.104113	412380.243766	51.716865
3360.673937	412076.962539	51.721869
3359.929886	411793.268741	51.726874
3359.099408	411491.899858	51.731879
3358.855024	411199.989908	51.736884
3357.800129	410912.423591	51.741889
3357.167973	410607.228161	51.746893
3356.676521	410309.910534	51.751898
3356.003207	410007.256754	51.756903
3355.656065	409709.834181	51.761908
3354.635425	409415.132707	51.766913
3353.962500	409115.062080	51.771917
3353.180802	408826.772040	51.776922
3352.692790	408535.611947	51.781927
3352.055759	408222.743903	51.786932
3351.097030	407931.906652	51.791937
3350.471672	407632.855972	51.796941
3350.033675	407342.769494	51.801946
3349.256015	407056.597041	51.806951
3348.717673	406765.529851	51.811956
3348.155067	406464.628093	51.816961
3347.181878	406158.603601	51.821965
3346.371851	405879.313022	51.826970
3345.827412	405588.693294	51.831975
3345.371572	405282.858006	51.836980
3344.363598	404999.981803	51.841985
3343.797615	404706.129441	51.846989
3343.089801	404414.330121	51.851994
3342.208293	404129.418188	51.856999
3341.869420	403830.895880	51.862004
3341.242748	403541.490345	51.867009
3340.728940	403254.885710	51.872013
3339.991427	402964.043651	51.877018
3339.193705	402664.312085	51.882023
3338.590922	402368.334248	51.887028
3337.587675	402082.177799	51.892033
3337.130426	401786.730815	51.897037
3336.137084	401493.145245	51.902042
3335.541968	401209.509285	51.907047
3334.663071	400919.484558	51.912052
3333.985389	400638.805350	51.917057
3333.775215	400335.502200	51.922061
3332.828571	400059.995403	51.927066
3332.211411	399775.791216	51.932071
3331.619878	399491.173786	51.937076
3330.818967	399205.824376	51.942081
3330.084465	398917.462299	51.947085
3329.393059	398621.108574	51.952090
3328.941602	398343.399147	51.957095
3328.184730	398059.990363	51.962100
3327.414384	397776.225390	51.967105
3327.054829	397497.807986	51.972109
3326.064851	397209.979954	51.977114
3325.189936	396919.716100	51.982119
3324.809475	396637.100115	51.987124
3323.692183	396365.911566	51.992129
3323.220735	396075.093597	51.997133
3322.974079	395791.864646	52.002138
3322.069068	395513.873041	52.007143
3321.611256	395219.409990	52.012148
3320.659981	394944.166840	52.017153
3320.246411	394650.047822	52.022157
3319.666812	394369.503851	52.027162
3318.811605	394081.577128	52.032167
3318.277143	393801.911258	52.037172
3317.603696	393520.663313	52.042177
3316.937408	393238.649187	52.047181
3316.586883	392947.251623	52.052186
3315.356591	392659.168976	52.057191
3314.716524	392373.965459	52.062196
3313.775556	392100.833824	52.067201
3313.713330	391809.559156	52.072205
3312.347912	391528.582553	52.077210
3311.815234	391240.606757	52.082215
3311.550529	390959.604112	52.087220
3310.599103	390679.699499	52.092225
3309.901287	390402.091900	52.097229
3309.288309	390117.450674	52.102234
3308.809468	389831.031439	52.107239
3308.352830	389556.303320	52.112244
3307.111976	389269.262680	52.117249
3306.718807	388987.145959	52.122253
3305.944705	388714.368741	52.127258
3305.039933	388436.880354	52.132263
3304.572358	388158.608686	52.137268
3303.976966	387888.924758	52.142273
3302.932453	387598.457701	52.147277
3302.689677	387327.086362	52.152282
3301.919178	387045.751675	52.157287
3301.054785	386763.793926	52.162292
3300.268031	386495.147179	52.167297
3299.669904	386214.541772	52.172301
3298.883637	385942.025492	52.177306
3298.270757	385672.455187	52.182311
3297.683449	385376.735821	52.187316
3297.022021	385111.492393	52.192321
3296.450296	384831.202955	52.197325
3295.442793	384567.866887	52.202330
3294.898980	384285.585287	52.207335
3294.531820	384008.843224	52.212340
3293.449107	383742.410568	52.217345
3293.323353	383458.072949	52.222349
3292.529560	383187.597821	52.227354
3291.608792	382921.311803	52.232359
3291.015494	382630.327705	52.237364
3290.250650	382368.260449	52.242369
3289.636208	382097.367723	52.247373
3288.815625	381829.761158	52.252378
3288.406470	381553.745454	52.257383
3288.069178	381275.223902	52.262388
3286.925657	381005.984064	52.267393
3286.508898	380733.320983	52.272397
3285.609339	380463.937065	52.277402
3284.851108	380187.509021	52.282407
3284.519038	379909.282067	52.287412
3283.658557	379639.250415	52.292417
3283.091700	379365.558699	52.297421
3282.155262	379092.305058	52.302426
3281.541623	378820.906126	52.307431
3281.006776	378546.567786	52.312436
3279.886054	378288.217516	52.317441
3279.377607	378009.140253	52.322445
3278.810829	377743.551364	52.327450
3277.876657	377471.329096	52.332455
3277.557660	377204.807180	52.337460
3276.922897	376937.137921	52.342465
3276.500978	376663.557342	52.347469
3275.774482	376398.315508	52.352474
3274.960024	376125.378423	52.357479
3274.333614	375852.002769	52.362484
3273.485448	375589.878244	52.367489
3273.100841	375308.880368	52.372493
3272.454675	375037.766336	52.377498
3271.362237	374775.090166	52.382503
3271.011432	374502.679439	52.387508
3270.251661	374238.827967	52.392513
3269.515749	373966.525496	52.397517
3268.671110	373691.567387	52.402522
3267.930418	373427.784063	52.407527
3267.510899	373159.445594	52.412532
3266.656500	372886.086378	52.417537
3266.160236	372625.795373	52.422541
3265.676996	372349.550217	52.427546
3264.720875	372091.262039	52.432551
3264.057365	371822.597493	52.437556
3263.499584	371551.701259	52.442561
3263.269538	371286.424590	52.447565
3262.171628	371014.567334	52.452570
3261.143756	370753.026048	52.457575
3260.828322	370487.503536	52.462580
3259.691517	370226.790375	52.467585
3259.296038	369959.216581	52.472589
3258.843896	369702.615144	52.477594
3258.058733	369429.553592	52.482599
3257.522520	369162.531415	52.487604
3256.609484	368902.003884	52.492609
3255.827965	368624.077413	52.497613
3255.172289	368365.032483	52.502618
3254.567651	368099.770142	52.507623
3254.604269	367830.079640	52.512628
3253.390847	367577.326166	52.517633
3252.781487	367302.875179	52.522637
3252.153440	367042.902231	52.527642
3251.404889	366784.295291	52.532647
3250.964363	366508.896794	52.537652
3250.201045	366246.879763	52.542657
3249.992890	365970.525276	52.547661
3249.138143	365706.102478	52.552666
3248.427524	365448.575942	52.557671
3247.613424	365166.002442	52.562676
3246.872824	364897.918470	52.567681
3246.161553	364631.965572	52.572685
3245.659682	364367.759092	52.577690
3244.834448	364103.347802	52.582695
3244.404875	363826.506502	52.587700
3243.684264	363552.712025	52.592705
3243.169935	363281.605879	52.597709
3242.015504	363028.385259	52.602714
3241.503229	362757.326635	52.607719
3240.968986	362483.063850	52.612724
3239.910975	362228.500523	52.617729
3239.199963	361955.942012	52.622733
3238.780962	361690.180567	52.627738
3238.119044	361431.962502	52.632743
3237.466947	361162.647156	52.637748
3236.663263	360904.066974	52.642753
3236.417907	360626.261699	52.647757
3235.272458	360364.577368	52.652762
3234.654247	360116.930903	52.657767
3234.188492	359842.769351	52.662772
3233.461276	359589.793689	52.667777
3232.959207	359317.187158	52.672781
3232.251796	359046.800014	52.677786
3231.466133	358786.144497	52.682791
3230.855713	358519.810624	52.687796
3230.065496	358263.555411	52.692801
3229.558154	357988.270391	52.697805
3228.350850	357724.164231	52.702810
3227.527044	357473.534153	52.707815
3227.413816	357205.078776	52.712820
3226.499827	356947.665776	52.717825
3225.617144	356696.303138	52.722829
3225.350736	356429.063908	52.727834
3224.655262	356179.679494	52.732839
3223.963694	355914.947843	52.737844
3223.475535	355650.284435	52.742849
3223.039637	355387.596389	52.747853
3222.489608	355114.770975	52.752858
3221.533752	354856.692352	52.757863
3220.852647	354586.836955	52.762868
3220.447507	354326.632649	52.767873
3219.425598	354062.350913	52.772877
3218.661191	353793.548000	52.777882
3217.815642	353528.803027	52.782887
3217.251489	353273.021409	52.787892
3216.498203	353018.846358	52.792897
3215.938869	352755.146568	52.797901
3215.551099	352492.563584	52.802906
3214.401156	352248.729425	52.807911
3214.270523	351973.352655	52.812916
3213.467862	351716.023353	52.817921
3212.860408	351456.065982	52.822925
3212.300838	351192.129475	52.827930
3211.664159	350934.948349	52.832935
3211.033175	350652.161446	52.837940
3210.248110	350406.581484	52.842945
3209.717469	350123.368755	52.847949
3209.204444	349852.470226	52.852954
3208.245177	349602.892918	52.857959
3207.472804	349329.309545	52.862964
3207.179839	349063.411755	52.867969
3206.302151	348800.964833	52.872973
3205.497836	348539.319534	52.877978
3204.744334	348274.916157	52.882983
3204.062938	348018.263045	52.887988
3203.339154	347752.249034	52.892993
3202.863873	347494.033805	52.897997
3201.997449	347232.188666	52.903002
3201.549076	346972.210597	52.908007
3200.741191	346718.549598	52.913012
3200.072729	346459.953025	52.918017
3199.533129	346196.066145	52.923021
3199.110054	345941.806352	52.928026
3198.276034	345662.360880	52.933031
3197.793378	345391.461715	52.938036
3196.872345	345130.659303	52.943041
3196.364332	344867.372313	52.948045
3195.869698	344594.511456	52.953050
3194.973974	344342.559443	52.958055
3194.468728	344068.806972	52.963060
3193.688398	343809.961905	52.968065
3193.004999	343547.027732	52.973069
3192.428744	343273.333778	52.978074
3191.681483	343011.578272	52.983079
3190.926120	342743.866579	52.988084
3190.262793	342495.204617	52.993089
3189.529301	342224.559917	52.998093
3189.175557	341949.603004	53.003098
3188.077782	341695.711943	53.008103
3187.740340	341413.673612	53.013108
3187.198529	341155.135947	53.018113
3186.297722	340895.279423	53.023117
3185.663372	340625.401186	53.028122
3184.940575	340372.565466	53.033127
3184.216463	340095.317091	53.038132
3183.730808	339839.768901	53.043137
3182.661937	339581.791834	53.048141
3182.205098	339322.215010	53.053146
3181.375016	339059.030529	53.058151
3181.187825	338792.128513	53.063156
3180.096300	338536.441890	53.068161
3179.344790	338277.492986	53.073165
3179.106348	338015.305302	53.078170
3178.448201	337748.855372	53.083175
3177.935209	337473.777084	53.088180
3176.989414	337226.870280	53.093185
3176.406367	336951.673629	53.098189
3176.019923	336678.557663	53.103194
3174.965616	336431.334147	53.108199
3174.318995	336158.155401	53.113204
3173.565181	335894.589861	53.118209
3172.986778	335623.078341	53.123213
3172.225166	335387.693259	53.128218
3171.482320	335118.853320	53.133223
3171.162551	334853.534913	53.138228
3170.103100	334595.944346	53.143233
3169.313237	334335.484366	53.148237
3169.269435	334062.660166	53.153242
3168.119952	333801.287693	53.158247
3167.664774	333534.280017	53.163252
3166.955754	333284.037479	53.168257
3166.732089	333013.987161	53.173261
3165.957428	332751.915069	53.178266
3165.244029	332498.895518	53.183271
3164.618468	332219.689856	53.188276
3163.644923	331959.683029	53.193281
3163.123168	331696.752426	53.198285
3162.498411	331427.039682	53.203290
3161.703129	331169.853228	53.208295
3161.078126	330909.329275	53.213300
3160.169491	330649.740346	53.218305
3159.798302	330380.034589	53.223309
3158.978551	330121.600883	53.228314
3158.403835	329865.393402	53.233319
3157.849243	329592.531426	53.238324
3157.243735	329330.802321	53.243329
3156.463258	329069.481895	53.248333
3156.030489	328799.423825	53.253338
3154.865363	328535.565555	53.258343
3154.622830	328269.014441	53.263348
3153.908381	328009.538555	53.268353
3153.160757	327745.637017	53.273357
3152.670382	327466.061399	53.278362
3151.661033	327208.920940	53.283367
3151.141330	326934.185521	53.288372
3150.458325	326673.630949	53.293377
3149.863024	326408.453319	53.298381
3149.195998	326151.993662	53.303386
3148.399956	325888.577405	53.308391
3147.826636	325622.808139	53.313396
3147.369779	325363.537541	53.318401
3146.420350	325091.129884	53.323405
3145.906595	324826.290681	53.328410
3144.910350	324568.885202	53.333415
3144.520811	324306.341650	53.338420
3144.103451	324046.347798	53.343425
3143.103219	323775.522498	53.348429
3142.394583	323506.738031	53.353434
3141.822443	323248.039299	53.358439
3141.243559	322976.304584	53.363444
3140.385092	322721.443338	53.368449
3139.613009	322464.581673	53.373453
3139.221642	322199.816815	53.378458
3138.259346	321940.106540	53.383463
3137.970867	321676.622388	53.388468
3137.087660	321418.425787	53.393473
3136.565460	321146.345458	53.398477
3136.168422	320876.994411	53.403482
3135.180508	320622.198553	53.408487
3134.341363	320347.568838	53.413492
3134.054787	320095.053997	53.418497
3133.277009	319834.952012	53.423501
3132.702090	319554.778262	53.428506
3131.555533	319297.126594	53.433511
3131.449554	319037.527198	53.438516
3130.615421	318769.181296	53.443521
3129.876219	318514.162085	53.448525
3129.426089	318241.068801	53.453530
3128.501717	317979.355291	53.458535
3128.364152	317719.222601	53.463540
3127.240810	317452.242864	53.468545
3126.417503	317183.890850	53.473549
3126.064124	316922.007781	53.478554
3125.088268	316656.632201	53.483559
3124.555278	316388.435813	53.488564
3123.767178	316132.144991	53.493569
3123.334315	315872.538000	53.498573
3122.541822	315610.975637	53.503578
3121.905118	315337.776588	53.508583
3121.208462	315078.107475	53.513588
3120.586859	314826.039474	53.518593
3119.668471	314549.725434	53.523597
3119.432349	314292.502417	53.528602
3118.336460	314043.155826	53.533607
3117.982041	313771.588659	53.538612
3117.154836	313513.031315	53.543617
3116.492230	313250.220281	53.548621
3115.965090	312985.808407	53.553626
3115.257391	312738.536380	53.558631
3114.634999	312468.867259	53.563636
3113.885587	312204.361370	53.568641
3113.141164	311939.217460	53.573645
3112.739891	311665.768169	53.578650
3111.925871	311413.697280	53.583655
3111.528686	311138.463572	53.588660
3110.627491	310890.275939	53.593665
3109.654616	310618.722596	53.598669
3109.113099	310364.212638	53.603674
3108.339706	310103.423569	53.608679
3107.814507	309837.399839	53.613684
3106.981550	309590.828433	53.618689
3106.138958	309330.583399	53.623693
3105.909771	309062.295683	53.628698
3104.970672	308816.936362	53.633703
3104.505295	308558.972789	53.638708
3104.147756	308285.941737	53.643713
3103.536302	308027.465418	53.648717
3102.726673	307771.999361	53.653722
3101.817883	307513.441723	53.658727
3101.265699	307243.113092	53.663732
3100.480845	306975.902026	53.668737
3099.910483	306733.128749	53.673741
3099.253226	306451.712191	53.678746
3098.410326	306200.832115	53.683751
3097.791473	305939.169648	53.688756
3096.995563	305679.953928	53.693761
3096.276116	305432.465292	53.698765
3095.994265	305166.724449	53.703770
3094.935613	304916.003489	53.708775
3094.320725	304655.280198	53.713780
3094.002244	304401.690895	53.718785
3092.963316	304151.907701	53.723789
3092.803090	303875.347654	53.728794
3092.063760	303624.726701	53.733799
3091.266285	303366.067255	53.738804
3090.833048	303099.735364	53.743809
3090.289840	302834.133455	53.748813
3089.493869	302564.420091	53.753818
3088.867816	302308.100058	53.758823
3088.627171	302035.267412	53.763828
3087.434310	301769.333538	53.768833
3086.694088	301519.498717	53.773837
3086.448823	301252.420840	53.778842
3085.581337	300978.004785	53.783847
3084.699680	300714.388292	53.788852
3084.268437	300455.767937	53.793857
3083.495834	300181.513804	53.798861
3082.630821	299921.611536	53.803866
3081.899534	299657.663982	53.808871
3081.287158	299391.379740	53.813876
3080.907907	299138.835684	53.818881
3079.755834	298878.467938	53.823885
3079.810607	298597.917412	53.828890
3078.924647	298350.953245	53.833895
3077.914014	298072.353174	53.838900
3077.238302	297814.735334	53.843905
3076.760104	297550.031544	53.848909
3075.729898	297294.837510	53.853914
3075.034509	297046.950112	53.858919
3074.746477	296785.042003	53.863924
3074.121681	296516.285260	53.868929
3073.278282	296274.023057	53.873933
3072.675016	296000.932806	53.878938
3072.049171	295747.608277	53.883943
3071.706768	295484.535582	53.888948
3070.766966	295222.499379	53.893953
3070.233807	294968.242414	53.898957
3069.648469	294700.062800	53.903962
3068.709017	294432.499173	53.908967
3068.065299	294173.623722	53.913972
3067.746872	293906.292259	53.918977
3066.447636	293660.533781	53.923981
3066.180100	293390.239440	53.928986
3065.604366	293123.253394	53.933991
3065.027713	292868.975470	53.938996
3064.272760	292603.392448	53.944001
3063.493627	292343.670499	53.949005
3063.202635	292071.239114	53.954010
3062.264832	291823.256817	53.959015
3061.622045	291535.396229	53.964020
3060.932651	291274.181864	53.969025
3060.128554	291021.542533	53.974029
3059.539612	290748.240079	53.979034
3058.957242	290475.038184	53.984039
3058.463488	290225.889021	53.989044
3057.646461	289959.574586	53.994049
3057.019740	289702.703809	53.999053
3056.499082	289420.832096	54.004058
3055.782791	289165.248422	54.009063
3055.139250	288896.817221	54.014068
3054.333145	288636.612174	54.019073
3053.555831	288375.510984	54.024077
3052.866295	288103.291678	54.029082
3052.159876	287850.379524	54.034087
3051.685342	287583.474041	54.039092
3050.779526	287316.713012	54.044097
3050.169230	287049.472059	54.049101
3049.853813	286782.719072	54.054106
3048.989136	286526.520182	54.059111
3048.308650	286268.279996	54.064116
3047.553568	286000.577322	54.069121
3046.923017	285740.189573	54.074125
3046.501944	285472.102608	54.079130
3045.491476	285214.474276	54.084135
3045.132979	284948.949363	54.089140
3044.348866	284688.839962	54.094145
3043.639110	284424.745613	54.099149
3043.094245	284151.405543	54.104154
3042.331842	283908.050341	54.109159
3041.808472	283629.791224	54.114164
3041.115001	283369.946931	54.119169
3040.284098	283106.660586	54.124173
3039.785303	282833.898310	54.129178
3038.875138	282563.213003	54.134183
3038.279192	282308.268168	54.139188
3037.653093	282033.691966	54.144193
3036.861050	281778.777959	54.149197
3036.600506	281511.249341	54.154202
3035.883928	281260.092510	54.159207
3034.930519	280987.146737	54.164212
3034.340153	280717.505231	54.169217
3033.684968	280458.774341	54.174221
3033.091465	280203.319029	54.179226
3032.407416	279935.576770	54.184231
3031.932679	279664.745110	54.189236
3031.187889	279404.882046	54.194241
3030.508351	279146.027330	54.199245
3030.012550	278867.558310	54.204250
3029.065851	278607.141263	54.209255
3028.303907	278346.924145	54.214260
3027.836543	278079.401876	54.219265
3026.993885	277828.442476	54.224269
3026.525088	277556.819953	54.229274
3025.720308	277293.706079	54.234279
3025.327140	277032.488101	54.239284
3024.227475	276774.667343	54.244289
3023.526112	276506.876327	54.249293
3023.383916	276237.214013	54.254298
3022.346784	275983.279989	54.259303
3021.732510	275724.236296	54.264308
3021.088523	275459.976288	54.269313
3020.338272	275195.325611	54.274317
3019.732068	274932.867896	54.279322
3018.957100	274672.397974	54.284327
3018.437258	274402.820947	54.289332
3017.640023	274137.795753	54.294337
3016.955892	273882.277862	54.299341
3016.669099	273613.810116	54.304346
3015.681829	273357.907310	54.309351
3015.021027	273094.694388	54.314356
3014.274390	272835.315353	54.319361
3013.427240	272569.355972	54.324365
3012.811025	272307.689716	54.329370
3012.449332	272069.210369	54.334375
3011.769803	271791.076235	54.339380
3011.076046	271531.994744	54.344385
3010.064196	271268.201093	54.349389
3009.669886	271005.685069	54.354394
3008.848390	270761.828606	54.359399
3008.202974	270492.959943	54.364404
3007.479685	270233.450564	54.369409
3006.906249	269984.894391	54.374413
3006.289511	269721.573560	54.379418
3005.589551	269472.579170	54.384423
3004.960637	269200.091902	54.389428
3004.283739	268937.519496	54.394433
3003.360376	268667.855111	54.399437
3003.040613	268411.746284	54.404442
3002.324414	268149.715294	54.409447
3001.402388	267889.983682	54.414452
3001.236829	267632.577413	54.419457
3000.401940	267379.606808	54.424461
2999.830697	267115.235808	54.429466
2998.654093	266859.492602	54.434471
2997.987589	266596.308512	54.439476
2997.617597	266336.592247	54.444481
2996.667237	266087.206174	54.449485
2996.334304	265830.998950	54.454490
2995.761350	265582.444828	54.459495
2995.066071	265326.473554	54.464500
2994.546196	265050.253070	54.469505
2993.862027	264807.600163	54.474509
2993.288700	264532.636454	54.479514
2992.305729	264280.608036	54.484519
2991.802674	264026.644674	54.489524
2991.450546	263752.461535	54.494529
2990.655216	263498.697635	54.499533
2989.937424	263234.199673	54.504538
2989.429036	262972.011826	54.509543
2988.833959	262705.559318	54.514548
2988.253487	262433.934756	54.519553
2987.428562	262181.730133	54.524557
2986.809505	261899.517551	54.529562
2986.201929	261643.866301	54.534567
2985.470979	261369.847097	54.539572
2984.884977	261101.611856	54.544577
2983.813441	260847.028007	54.549581
2983.553794	260576.551399	54.554586
2983.028283	260314.623339	54.559591
2982.234359	260045.021339	54.564596
2981.471678	259776.433378	54.569601
2980.885962	259514.082710	54.574605
2980.394364	259248.508510	54.579610
2979.676343	258973.802135	54.584615
2978.805916	258704.009951	54.589620
2978.189676	258437.081127	54.594625
2977.279077	258180.462570	54.599629
2976.711367	257905.937382	54.604634
2976.064317	257641.764831	54.609639
2975.338401	257385.347144	54.614644
2975.168707	257121.761799	54.619649
2974.167684	256850.897389	54.624653
2973.460434	256581.285648	54.629658
2972.886489	256325.660111	54.634663
2972.597849	256047.069270	54.639668
2972.140521	255781.748418	54.644673
2971.091891	255510.867813	54.649677
2970.653505	255239.458036	54.654682
2969.942390	254956.911774	54.659687
2969.018892	254683.542191	54.664692
2968.393242	254424.692950	54.669697
2967.771466	254152.447843	54.674701
2967.079722	253883.270232	54.679706
2966.352997	253615.626560	54.684711
2965.458790	253350.658337	54.689716
2965.013490	253075.330864	54.694721
2963.891082	252816.537042	54.699725
2963.244488	252549.926402	54.704730
2962.753692	252277.637906	54.709735
2962.080747	252017.067850	54.714740
2961.219741	251748.302254	54.719745
2960.589265	251486.172826	54.724749
2960.109456	251215.463212	54.729754
2959.467274	250952.878079	54.734759
2958.726125	250697.134032	54.739764
2958.291723	250426.062003	54.744769
2957.243230	250180.299315	54.749773
2956.902171	249904.018260	54.754778
2956.365858	249650.535429	54.759783
2955.642971	249375.945589	54.764788
2954.861604	249112.137682	54.769793
2953.919074	248852.124730	54.774797
2953.764335	248572.251307	54.779802
2953.013707	248320.892825	54.784807
2952.265516	248055.808217	54.789812
2951.823181	247767.934586	54.794817
2951.078674	247519.250430	54.799821
2950.478795	247240.366781	54.804826
2949.689336	246970.681373	54.809831
2949.220456	246710.495386	54.814836
2948.806301	246433.926774	54.819841
2947.668103	246164.807438	54.824845
2947.064774	245895.578491	54.829850
2946.213209	245628.401150	54.834855
2945.443219	245380.106825	54.839860
2945.146003	245102.121797	54.844865
2944.218095	244840.178531	54.849869
2943.507577	244575.858559	54.854874
2943.027204	244309.287209	54.859879
2942.279938	244032.878144	54.864884
2941.514719	243773.636052	54.869889
2940.978740	243514.765640	54.874893
2940.443109	243238.426657	54.879898
2939.793462	242976.061166	54.884903
2939.042772	242717.430112	54.889908
2938.684093	242444.120678	54.894913
2938.068106	242173.450005	54.899917
2937.292918	241901.124461	54.904922
2936.367999	241633.508750	54.909927
2935.723614	241367.606292	54.914932
2935.362539	241087.908680	54.919937
2934.373722	240836.805966	54.924941
2933.909041	240559.086790	54.929946
2933.175416	240292.869862	54.934951
2932.472277	240023.771247	54.939956
2931.797208	239756.705970	54.944961
2931.299918	239485.742609	54.949965
2930.457783	239210.760221	54.954970
2929.804218	238952.554997	54.959975
2929.422265	238671.898977	54.964980
2928.912225	238401.449560	54.969985
2927.930653	238135.073305	54.974989
2927.103603	237858.615003	54.979994
2926.639926	237599.517148	54.984999
2925.732823	237318.234784	54.990004
2925.233080	237054.178531	54.995009
2924.582123	236786.429188	55.000013
2923.969561	236520.125876	55.005018
2923.159021	236253.218001	55.010023
2922.151673	235981.427530	55.015028
2921.700827	235718.614640	55.020033
2921.047539	235454.433995	55.025037
2920.765871	235179.398793	55.030042
2919.826263	234921.095958	55.035047
2919.308477	234654.935299	55.040052
2918.871647	234377.813431	55.045057
2918.168384	234114.713692	55.050061
2917.371837	233846.129443	55.055066
2916.474262	233573.131398	55.060071
2915.989458	233291.538754	55.065076
2915.610995	233017.619828	55.070081
2914.594128	232757.858120	55.075085
2914.193514	232489.902472	55.080090
2913.249076	232215.795380	55.085095
2912.515645	231942.623255	55.090100
2911.932317	231681.089908	55.095105
2911.250827	231417.077542	55.100109
2910.888612	231134.886323	55.105114
2909.963626	230874.020456	55.110119
2909.174924	230607.455732	55.115124
2909.172194	230318.946477	55.120129
2908.137859	230059.398836	55.125133
2907.618936	229785.027975	55.130138
2906.933746	229514.121618	55.135143
2906.290702	229234.577929	55.140148
2905.426893	228955.121007	55.145153
2904.706092	228688.627686	55.150157
2904.421028	228413.816710	55.155162
2903.463514	228154.644470	55.160167
2902.916944	227866.993225	55.165172
2902.635773	227594.450310	55.170177
2901.592176	227327.706799	55.175181
2900.865572	227043.702326	55.180186
2900.338715	226775.771204	55.185191
2899.543527	226507.234177	55.190196
2898.767166	226216.455099	55.195201
2898.112200	225953.180775	55.200205
2897.600972	225684.181375	55.205210
2896.981261	225402.635298	55.210215
2896.231882	225141.899131	55.215220
2895.686237	224858.560998	55.220225
2894.973542	224583.664913	55.225229
2894.220845	224306.650190	55.230234
2893.641252	224040.264051	55.235239
2892.898571	223761.263772	55.240244
2892.326016	223492.383301	55.245249
2891.533526	223215.467834	55.250253
2890.970355	222952.456219	55.255258
2889.877370	222667.252246	55.260263
2889.265709	222410.602326	55.265268
2889.174051	222138.315236	55.270273
2888.045441	221871.361542	55.275277
2887.462370	221594.622451	55.280282
2887.145264	221320.159047	55.285287
2886.521887	221056.196076	55.290292
2885.666453	220768.708527	55.295297
2884.919963	220502.475711	55.300301
2884.242787	220218.424481	55.305306
2883.550685	219956.996731	55.310311
2883.056234	219683.407614	55.315316
2882.557116	219397.447450	55.320321
2881.617721	219134.979826	55.325325
2880.732731	218862.855858	55.330330
2880.419796	218588.389298	55.335335
2879.697177	218319.296672	55.340340
2878.911099	218046.625538	55.345345
2878.228238	217773.137190	55.350349
2877.739638	217489.474219	55.355354
2877.135672	217229.442668	55.360359
2876.281953	216958.301207	55.365364
2875.824166	216673.758392	55.370369
2875.392561	216396.595246	55.375373
2874.346996	216128.873252	55.380378
2873.569227	215853.714594	55.385383
2873.369807	215583.556890	55.390388
2872.738390	215306.200697	55.395393
2872.004423	215036.829884	55.400397
2871.219199	214747.281050	55.405402
2870.605752	214468.436252	55.410407
2869.653904	214204.309180	55.415412
2869.491772	213920.953053	55.420417
2868.690521	213645.056222	55.425421
2867.944955	213364.455059	55.430426
2867.140294	213093.117759	55.435431
2866.450196	212810.028227	55.440436
2866.096963	212531.481384	55.445441
2865.246418	212256.934681	55.450445
2864.735585	211983.239039	55.455450
2864.050567	211698.753529	55.460455
2862.998969	211420.907573	55.465460
2862.852524	211145.172310	55.470465
2862.149218	210869.602792	55.475469
2861.322915	210594.753974	55.480474
2860.439211	210320.335461	55.485479
2860.033148	210040.344266	55.490484
2859.561169	209759.881131	55.495489
2858.491264	209486.641256	55.500493
2857.818095	209204.341587	55.505498
2857.302712	208924.436407	55.510503
2856.188181	208658.639990	55.515508
2855.718519	208385.360902	55.520513
2855.156720	208116.221201	55.525517
2854.282565	207833.692458	55.530522
2853.756787	207573.331108	55.535527
2853.053195	207285.127185	55.540532
2852.847689	207023.037574	55.545537
2851.847057	206750.931798	55.550541
2851.155914	206467.718767	55.555546
2850.736370	206190.038359	55.560551
2849.542099	205924.763093	55.565556
2849.228485	205639.610749	55.570561
2848.734844	205368.856480	55.575565
2847.482190	205090.486015	55.580570
2846.884279	204821.583423	55.585575
2846.398779	204551.684365	55.590580
2845.893602	204278.366342	55.595585
2845.220074	204013.055589	55.600589
2844.369442	203740.800217	55.605594
2844.225306	203460.391426	55.610599
2843.000864	203186.390822	55.615604
2842.438141	202912.503113	55.620609
2841.712827	202644.801801	55.625613
2841.336494	202365.682386	55.630618
2840.519088	202088.912121	55.635623
2839.603936	201827.314981	55.640628
2839.185001	201551.935035	55.645633
2838.567635	201284.375918	55.650637
2838.063802	201012.855233	55.655642
2837.563015	200731.078739	55.660647
2837.079357	200457.216157	55.665652
2836.121281	200172.919007	55.670657
2835.527785	199903.085088	55.675661
2834.723797	199618.601038	55.680666
2833.850896	199349.501308	55.685671
2833.116732	199060.822619	55.690676
2832.973582	198791.508349	55.695681
2832.201659	198525.565312	55.700685
2831.507961	198245.194010	55.705690
2830.905801	197969.097948	55.710695
2830.203002	197685.600789	55.715700
2829.964855	197410.378933	55.720705
2829.099512	197124.251124	55.725709
2828.496305	196835.971121	55.730714
2827.879992	196565.674383	55.735719
2826.985043	196283.678627	55.740724
2826.384389	195995.313858	55.745729
2825.725810	195714.467163	55.750733
2825.346780	195431.401923	55.755738
2824.626442	195146.331014	55.760743
2823.437116	194860.865195	55.765748
2822.999486	194586.351756	55.770753
2822.257027	194305.984229	55.775757
2821.307321	194013.614411	55.780762
2820.836752	193745.765328	55.785767
2820.310530	193469.452567	55.790772
2820.329769	193181.107553	55.795777
2818.833359	192907.712583	55.800781
2818.074263	192625.016072	55.805786
2817.861393	192342.909025	55.810791
2816.919383	192059.634027	55.815796
2816.292026	191777.977585	55.820801
2815.448320	191507.527933	55.825805
2814.922036	191230.731619	55.830810
2814.731634	190950.333995	55.835815
2813.579167	190677.533256	55.840820
2813.309178	190385.446474	55.845825
2812.500082	190109.617459	55.850829
2811.747498	189827.165306	55.855834
2811.280670	189539.936777	55.860839
2810.540396	189263.923667	55.865844
2809.839696	188973.096986	55.870849
2809.197123	188690.748716	55.875853
2808.841774	188405.150647	55.880858
2807.959783	188125.731665	55.885863
2807.070936	187842.295256	55.890868
2806.352084	187553.935670	55.895873
2805.359749	187281.256500	55.900877
2805.073217	186999.867164	55.905882
2804.614753	186722.590486	55.910887
2803.525527	186441.280814	55.915892
2803.080881	186156.245122	55.920897
2802.427380	185884.258473	55.925901
2801.893802	185614.875096	55.930906
2801.163169	185315.591005	55.935911
2800.153868	185041.744841	55.940916
2799.530257	184748.948181	55.945921
2798.962765	184484.589123	55.950925
2798.227880	184208.707369	55.955930
2797.801848	183930.615836	55.960935
2796.933896	183646.375489	55.965940
2796.763957	183370.791102	55.970945
2795.995619	183096.104617	55.975949
2795.124708	182805.089979	55.980954
2794.750958	182534.936689	55.985959
2793.639726	182253.911312	55.990964
2793.163333	181966.287049	55.995969
2792.397658	181690.743986	56.000973
2791.675239	181404.828781	56.005978
2791.480538	181126.044255	56.010983
2790.495075	180844.435699	56.015988
2789.888256	180555.760276	56.020993
2789.079993	180288.373767	56.025997
2788.500486	180004.086136	56.031002
2787.902197	179720.057775	56.036007
2786.957322	179437.803369	56.041012
2786.265144	179158.156508	56.046017
2785.491367	178878.677061	56.051021
2784.912345	178604.345447	56.056026
2784.659904	178330.345486	56.061031
2783.575212	178050.017730	56.066036
2783.005967	177775.308429	56.071041
2782.495063	177504.967083	56.076045
2781.742989	177215.841516	56.081050
2781.334936	176935.083430	56.086055
2780.376442	176661.028246	56.091060
2779.823221	176375.858083	56.096065
2779.324251	176096.239379	56.101069
2778.408736	175831.047869	56.106074
2778.262791	175547.396088	56.111079
2777.530686	175258.777188	56.116084
2776.820630	174961.203141	56.121089
2775.881130	174702.305666	56.126093
2775.226379	174411.200509	56.131098
2774.588192	174128.221686	56.136103
2773.937572	173858.448099	56.141108
2773.424530	173575.135416	56.146113
2772.492244	173292.196375	56.151117
2771.794103	173021.749218	56.156122
2771.265572	172741.242831	56.161127
2770.530806	172456.739639	56.166132
2770.025797	172168.806552	56.171137
2769.468695	171899.018773	56.176141
2768.866943	171621.685865	56.181146
2768.197150	171323.369645	56.186151
2767.257776	171046.234189	56.191156
2766.639687	170754.196379	56.196161
2766.205693	170476.514415	56.201165
2765.485187	170200.545725	56.206170
2764.896485	169926.669108	56.211175
2764.292537	169643.310257	56.216180
2763.673263	169348.714519	56.221185
2762.825922	169072.570558	56.226189
2762.307270	168789.713175	56.231194
2761.960210	168505.050443	56.236199
2761.037416	168152.754909	56.241204
2760.580491	167860.357586	56.246209
2759.929462	167572.558289	56.251213
2759.197101	167270.138160	56.256218
2758.814797	166998.793122	56.261223
2757.523747	166699.454287	56.266228
2757.085109	166422.616486	56.271233
2756.446174	166138.462945	56.276237
2755.831480	165826.359429	56.281242
2755.498047	165538.639948	56.286247
2754.647451	165266.288216	56.291252
2754.008990	164968.284091	56.296257
2753.232706	164664.188331	56.301261
2752.013176	164374.393195	56.306266
2751.833739	164096.489179	56.311271
2751.069669	163811.508829	56.316276
2750.823802	163523.982014	56.321281
2749.658645	163236.437800	56.326285
2749.379954	162948.526604	56.331290
2748.526298	162650.817106	56.336295
2747.872453	162356.765519	56.341300
2746.874351	162074.302486	56.346305
2746.450429	161789.665651	56.351309
2745.887566	161500.641398	56.356314
2744.883428	161200.412323	56.361319
2744.014455	160932.863779	56.366324
2743.441475	160639.767061	56.371329
2743.055170	160343.274153	56.376333
2742.221520	160068.594338	56.381338
2741.769711	159775.498324	56.386343
2740.660535	159514.189921	56.391348
2740.443536	159201.152804	56.396353
2739.625505	158927.903312	56.401357
2738.979211	158641.305762	56.406362
2738.321007	158373.387393	56.411367
2737.784967	158078.259529	56.416372
2736.981454	157783.049427	56.421377
2736.408386	157512.085968	56.426381
2735.590152	157236.065856	56.431386
2735.133757	156947.469169	56.436391
2734.273205	156659.777928	56.441396
2733.508949	156384.696822	56.446401
2732.790041	156091.661629	56.451405
2732.343784	155788.352830	56.456410
2731.704668	155535.440747	56.461415
2731.119008	155238.502058	56.466420
2730.569869	154948.881969	56.471425
2729.579484	154675.668294	56.476429
2729.154094	154382.118400	56.481434
2728.237059	154083.615365	56.486439
2727.478383	153832.730666	56.491444
2726.740345	153524.899829	56.496449
2726.131898	153256.899551	56.501453
2725.645112	152974.963987	56.506458
2725.074982	152694.022736	56.511463
2724.380770	152418.797810	56.516468
2723.796853	152128.063806	56.521473
2722.847002	151831.124198	56.526477
2722.371408	151566.713589	56.531482
2722.050049	151270.327719	56.536487
2721.142420	150986.493099	56.541492
2720.505174	150710.193152	56.546497
2719.857093	150417.743273	56.551501
2718.942023	150143.335060	56.556506
2718.534986	149843.989011	56.561511
2717.295427	149558.249506	56.566516
2716.849795	149297.347688	56.571521
2716.219042	149003.738618	56.576525
2715.593231	148723.946136	56.581530
2715.095061	148458.725690	56.586535
2714.555147	148172.824152	56.591540
2713.347765	147886.636945	56.596545
2712.984228	147599.721338	56.601549
2712.510282	147320.997343	56.606554
2711.876035	147050.269319	56.611559
2711.038554	146775.547303	56.616564
2710.207724	146467.582224	56.621569
2709.719928	146194.207778	56.626573
2708.934169	145922.573062	56.631578
2708.548621	145631.459841	56.636583
2707.874773	145346.240517	56.641588
2707.253019	145071.664461	56.646593
2706.557931	144788.575769	56.651597
2705.854766	144514.602073	56.656602
2705.213458	144203.909947	56.661607
2704.132701	143949.011020	56.666612
2703.979888	143656.049635	56.671617
2703.333464	143366.282406	56.676621
2702.263043	143094.501549	56.681626
2702.237952	142800.308247	56.686631
2700.952147	142541.730457	56.691636
2700.771551	142240.146595	56.696641
2699.759546	141956.308280	56.701645
2699.233562	141677.630548	56.706650
2698.673026	141384.920711	56.711655
2697.857972	141115.226272	56.716660
2697.344781	140827.202813	56.721665
2696.682953	140532.039669	56.726669
2695.827345	140242.398907	56.731674
2695.208401	139979.976550	56.736679
2694.336016	139710.138633	56.741684
2694.205273	139393.176522	56.746689
2693.099945	139141.244119	56.751693
2692.421878	138820.004278	56.756698
2691.994238	138558.974373	56.761703
2691.199438	138257.426168	56.766708
2690.385373	138004.491730	56.771713
2690.007499	137684.982590	56.776717
2689.176909	137443.324421	56.781722
2688.772042	137125.896437	56.786727
2687.930459	136835.156076	56.791732
2687.250143	136572.494177	56.796737
2686.426637	136291.957630	56.801741
2685.480452	135998.167854	56.806746
2685.412652	135731.160766	56.811751
2684.283024	135433.531172	56.816756
2683.550740	135175.755550	56.821761
2683.492031	134872.436119	56.826765
2682.510392	134590.454822	56.831770
2682.128961	134328.998105	56.836775
2681.367201	134027.615481	56.841780
2680.583324	133757.246831	56.846785
2680.379880	133467.214096	56.851789
2679.363633	133180.107615	56.856794
2678.931538	132899.631015	56.861799
2678.390402	132604.655841	56.866804
2677.470180	132313.605219	56.871809
2676.887337	132049.902230	56.876813
2676.494384	131753.972495	56.881818
2675.796690	131468.928682	56.886823
2674.898782	131174.164681	56.891828
2674.214647	130888.006873	56.896833
2673.230222	130611.641456	56.901837
2672.493555	130338.097282	56.906842
2671.977667	130036.235585	56.911847
2671.237844	129754.340354	56.916852
2670.634027	129479.272155	56.921857
2669.912128	129195.906460	56.926861
2669.448602	128904.272790	56.931866
2668.842091	128613.896787	56.936871
2667.915692	128341.735888	56.941876
2667.358534	128063.004010	56.946881
2666.728034	127774.558377	56.951885
2666.027964	127490.724150	56.956890
2665.476333	127204.888189	56.961895
2664.676423	126939.604418	56.966900
2664.029107	126634.092502	56.971905
2663.417667	126368.771729	56.976909
2662.587879	126070.520982	56.981914
2662.158813	125808.757964	56.986919
2661.433692	125525.367266	56.991924
2660.549359	125229.648818	56.996929
2660.196642	124966.167527	57.001933
2659.238146	124667.635192	57.006938
2658.625667	124397.051352	57.011943
2658.340479	124101.390068	57.016948
2657.187660	123819.964452	57.021953
2656.977103	123555.230080	57.026957
2656.407134	123273.476619	57.031962
2655.457077	122974.111099	57.036967
2654.624547	122698.906571	57.041972
2653.775947	122413.625651	57.046977
2653.749105	122142.260866	57.051981
2652.670016	121844.363359	57.056986
2652.048178	121590.531777	57.061991
2651.229812	121278.886518	57.066996
2650.643308	121027.251344	57.072001
2650.122356	120734.521763	57.077005
2649.451966	120445.977243	57.082010
2648.887641	120171.397827	57.087015
2647.984615	119902.302617	57.092020
2647.872840	119598.126057	57.097025
2646.658842	119340.093466	57.102029
2646.363826	119050.006818	57.107034
2645.864299	118739.255492	57.112039
2645.297806	118474.882657	57.117044
2644.659890	118190.401598	57.122049
2643.674377	117882.962227	57.127053
2642.936001	117620.504299	57.132058
2642.556378	117325.924643	57.137063
2641.632118	117032.754934	57.142068
2641.295348	116751.504695	57.147073
2640.638670	116469.203815	57.152077
2639.819239	116182.488805	57.157082
2639.166060	115885.512752	57.162087
2638.122873	115602.946338	57.167092
2637.817130	115323.534936	57.172097
2636.835854	115031.692132	57.177101
2636.390732	114755.025586	57.182106
2635.798361	114444.823636	57.187111
2634.785116	114203.953805	57.192116
2634.464606	113883.091317	57.197121
2633.789968	113619.941197	57.202125
2633.030482	113310.719048	57.207130
2632.728215	113038.592887	57.212135
2631.976545	112753.219920	57.217140
2631.101199	112466.213445	57.222145
2630.347502	112177.045998	57.227149
2629.542144	111925.478240	57.232154
2629.406887	111613.766762	57.237159
2628.635875	111340.216792	57.242164
2627.749745	111056.452141	57.247169
2627.658152	110747.441704	57.252173
2626.371079	110469.687053	57.257178
2625.752173	110181.644851	57.262183
2625.131369	109889.602258	57.267188
2624.526675	109607.580202	57.272193
2623.733316	109330.394816	57.277197
2623.031472	109046.624260	57.282202
2622.464844	108752.010482	57.287207
2622.008741	108482.712965	57.292212
2621.078874	108202.097582	57.297217
2620.270272	107899.861199	57.302221
2619.679298	107629.020974	57.307226
2619.129830	107344.116816	57.312231
2618.501531	107046.602235	57.317236
2617.924125	106766.487031	57.322241
2616.933331	106478.109991	57.327245
2616.314407	106217.733509	57.332250
2616.118485	105922.270797	57.337255
2614.890000	105632.323763	57.342260
2614.087662	105369.492218	57.347265
2613.803890	105066.960971	57.352269
2613.030078	104779.699391	57.357274
2612.486177	104517.090102	57.362279
2611.774346	104230.434406	57.367284
2611.263472	103937.196954	57.372289
2610.768883	103654.960994	57.377293
2609.702031	103388.063458	57.382298
2609.450175	103082.260089	57.387303
2608.492913	102807.041408	57.392308
2607.932080	102520.065443	57.397313
2607.306888	102231.732985	57.402317
2606.551518	101952.908247	57.407322
2605.829622	101650.909023	57.412327
2605.494955	101393.630008	57.417332
2604.287128	101095.108698	57.422337
2604.005437	100809.511440	57.427341
2603.032158	100521.096777	57.432346
2602.841676	100226.846601	57.437351
2601.994857	99952.722532	57.442356
2601.140886	99671.923810	57.447361
2600.706669	99386.539586	57.452365
2599.858631	99098.021412	57.457370
2599.141702	98822.367994	57.462375
2598.469914	98532.769791	57.467380
2597.989566	98249.722075	57.472385
2597.112335	97975.436199	57.477389
2596.239740	97694.138277	57.482394
2595.816744	97403.056267	57.487399
2594.728925	97137.509093	57.492404
2593.937466	96840.309076	57.497409
2594.051995	96575.789295	57.502413
2593.061127	96305.416594	57.507418
2592.455958	96008.806820	57.512423
2591.915543	95722.965362	57.517428
2591.387270	95450.018282	57.522433
2590.672323	95170.838581	57.527437
2589.902716	94887.510969	57.532442
2589.118255	94596.040527	57.537447
2588.824327	94311.560444	57.542452
2587.716699	94057.999939	57.547457
2586.891691	93755.411581	57.552461
2586.313675	93475.914315	57.557466
2585.905866	93206.951457	57.562471
2584.855175	92940.376494	57.567476
2584.479179	92640.116401	57.572481
2584.054412	92389.979608	57.577485
2583.066477	92085.284002	57.582490
2582.487849	91806.752694	57.587495
2581.939649	91534.681142	57.592500
2581.201958	91263.169249	57.597505
2580.553080	90972.847297	57.602509
2579.840531	90671.392982	57.607514
2578.996826	90429.149855	57.612519
2578.529501	90128.418661	57.617524
2578.032404	89870.923077	57.622529
2577.244163	89585.333336	57.627533
2576.347195	89294.946231	57.632538
2575.617609	89031.867577	57.637543
2574.928190	88753.608335	57.642548
2574.506793	88489.054648	57.647553
2574.012414	88194.320196	57.652557
2573.244776	87928.864626	57.657562
2572.691353	87619.750322	57.662567
2571.850756	87334.731130	57.667572
2571.140243	87111.623524	57.672577
2570.750210	86807.712252	57.677581
2569.629390	86524.396437	57.682586
2569.176711	86262.239612	57.687591
2568.807100	85958.679481	57.692596
2567.844581	85711.430687	57.697601
2567.389176	85397.116077	57.702605
2566.704783	85157.005154	57.707610
2566.082087	84863.458878	57.712615
2564.974751	84575.431937	57.717620
2564.642120	84315.340130	57.722625
2564.284039	84014.987884	57.727629
2563.159265	83745.907728	57.732634
2562.719247	83470.251187	57.737639
2561.793042	83183.710369	57.742644
2561.141903	82915.795372	57.747649
2560.638397	82634.385918	57.752653
2560.187715	82370.527764	57.757658
2559.640383	82077.337977	57.762663
2558.837372	81818.118518	57.767668
2557.831038	81504.164843	57.772673
2557.577935	81251.855661	57.777677
2556.795338	80960.480715	57.782682
2556.204737	80675.334399	57.787687
2555.388638	80417.224516	57.792692
2554.523563	80104.473718	57.797697
2554.034074	79866.312758	57.802701
2553.270792	79563.858153	57.807706
2552.485210	79277.684739	57.812711
2551.974761	79012.503672	57.817716
2551.469523	78746.311320	57.822721
2550.843759	78461.955266	57.827725
2549.789768	78180.307048	57.832730
2549.329889	77894.196368	57.837735
2548.547144	77634.424303	57.842740
2548.268396	77347.842688	57.847745
2547.206127	77065.019949	57.852749
2546.233971	76795.163305	57.857754
2546.174101	76524.094865	57.862759
2545.437420	76248.359981	57.867764
2544.702648	75977.247419	57.872769
2544.516358	75700.710474	57.877773
2543.429207	75417.496516	57.882778
2542.789747	75139.594537	57.887783
2542.072083	74848.220410	57.892788
2541.225682	74580.540176	57.897793
2540.529043	74309.241282	57.902797
2540.209540	74019.412592	57.907802
2539.312521	73740.892921	57.912807
2538.557790	73480.080215	57.917812
2537.964351	73205.675725	57.922817
2537.596453	72920.393853	57.927821
2536.455252	72649.143619	57.932826
2535.943382	72379.381033	57.937831
2535.216303	72109.858931	57.942836
2534.512398	71840.881594	57.947841
2534.127346	71562.228932	57.952845
2533.192248	71293.960796	57.957850
2532.525531	71016.190284	57.962855
2531.657327	70751.656173	57.967860
2530.552756	70478.789328	57.972865
2530.566757	70193.403892	57.977869
2529.663736	69956.008472	57.982874
2528.887038	69669.185152	57.987879
2528.500346	69426.203828	57.992884
2527.939524	69139.379390	57.997889
2527.432161	68865.990651	58.002893
2526.329763	68613.043405	58.007898
2526.124451	68329.144965	58.012903
2525.513820	68050.273932	58.017908
2524.448291	67784.645887	58.022913
2523.973388	67505.881492	58.027917
2523.275083	67262.317906	58.032922
2522.491641	66966.409463	58.037927
2521.792521	66712.216643	58.042932
2521.020974	66449.581138	58.047937
2520.662419	66167.150891	58.052941
2519.754717	65903.844638	58.057946
2519.412580	65622.186041	58.062951
2518.533233	65364.708648	58.067956
2517.996571	65073.267257	58.072961
2517.223769	64836.968255	58.077965
2517.155000	64533.201573	58.082970
2515.929142	64289.901737	58.087975
2515.181175	64009.746421	58.092980
2514.663045	63725.898933	58.097985
2513.793008	63479.393415	58.102989
2513.124157	63206.949588	58.107994
2512.621794	62939.874709	58.112999
2512.041499	62674.582459	58.118004
2511.150710	62410.783560	58.123009
2510.827345	62142.010551	58.128013
2510.209340	61862.591300	58.133018
2509.277800	61586.780872	58.138023
2508.748412	61329.426153	58.143028
2508.155949	61051.344431	58.148033
2507.780406	60779.740664	58.153037
2506.548335	60513.512220	58.158042
2506.283893	60225.520929	58.163047
2505.621757	59962.995777	58.168052
2504.641625	59700.853909	58.173057
2504.311585	59427.857160	58.178061
2503.535587	59150.301242	58.183066
2502.690099	58886.759962	58.188071
2502.183959	58618.623529	58.193076
2501.575135	58342.892097	58.198081
2500.750409	58074.177854	58.203085
2499.845340	57820.295488	58.208090
2499.152769	57548.934665	58.213095
2498.621797	57272.814386	58.218100
2497.679088	57019.097750	58.223105
2497.266111	56744.894059	58.228109
2496.726435	56483.854556	58.233114
2495.708906	56234.746314	58.238119
2495.359356	55950.107237	58.243124
2494.672394	55696.558201	58.248129
2494.122966	55427.187039	58.253133
2493.164682	55167.751619	58.258138
2492.563646	54884.687944	58.263143
2492.143286	54636.715627	58.268148
2491.487564	54380.255980	58.273153
2491.010847	54105.775995	58.278157
2490.142783	53830.346453	58.283162
2489.271286	53563.879595	58.288167
2488.797399	53295.758874	58.293172
2487.481656	53028.500159	58.298177
2487.282494	52769.867762	58.303181
2486.637281	52505.665098	58.308186
2485.817433	52238.507162	58.313191
2485.371405	51986.968200	58.318196
2484.885298	51725.517056	58.323201
2484.077038	51447.077012	58.328205
2483.371045	51193.733165	58.333210
2482.674638	50922.746989	58.338215
2481.857017	50662.895146	58.343220
2481.293324	50397.131863	58.348225
2480.781374	50131.740804	58.353229
2479.985544	49873.276335	58.358234
2479.473644	49606.570699	58.363239
2478.833372	49341.841285	58.368244
2477.932740	49078.419300	58.373249
2477.111488	48815.377739	58.378253
2476.312235	48574.647751	58.383258
2475.890495	48297.634926	58.388263
2475.248714	48045.856705	58.393268
2474.453308	47790.569943	58.398273
2473.822748	47517.429941	58.403277
2473.073833	47274.229757	58.408282
2472.447826	47013.581705	58.413287
2471.795968	46746.479537	58.418292
2471.347416	46495.126169	58.423297
2470.306627	46232.898043	58.428301
2469.758524	45979.878828	58.433306
2469.051212	45734.321201	58.438311
2468.324661	45466.668402	58.443316
2467.790048	45216.979023	58.448321
2467.363435	44959.293414	58.453325
2466.437303	44705.289909	58.458330
2465.823477	44455.007279	58.463335
2465.104363	44196.749960	58.468340
2464.111242	43938.024426	58.473345
2463.554210	43682.339170	58.478349
2463.123484	43444.043687	58.483354
2462.425950	43177.496736	58.488359
2461.571581	42928.583490	58.493364
2460.758784	42682.317242	58.498369
2460.420718	42419.899221	58.503373
2459.277095	42184.902688	58.508378
2458.530169	41935.110817	58.513383
2458.131701	41681.725768	58.518388
2457.589189	41439.722265	58.523393
2457.010942	41191.868614	58.528397
2456.222263	40945.993358	58.533402
2455.160894	40697.059848	58.538407
2454.700201	40451.109667	58.543412
2453.882459	40211.797833	58.548417
2453.366341	39959.840209	58.553421
2452.308303	39724.029153	58.558426
2451.866184	39486.206145	58.563431
2451.183653	39236.424494	58.568436
2450.646442	39002.075861	58.573441
2449.901425	38763.242360	58.578445
2449.389197	38518.548625	58.583450
2449.088783	38277.899989	58.588455
2448.366943	38033.339757	58.593460
2447.410528	37791.116999	58.598465
2446.962877	37551.716011	58.603469
2446.161312	37306.115155	58.608474
2445.109379	37068.040256	58.613479
2444.776224	36820.156186	58.618484
2443.660797	36578.944970	58.623489
2443.446414	36349.209894	58.628493
2442.326697	36118.894443	58.633498
2441.617424	35872.866826	58.638503
2440.953802	35639.541158	58.643508
2440.197513	35414.772717	58.648513
2439.395136	35171.733551	58.653517
2438.848076	34941.163354	58.658522
2438.186302	34720.063769	58.663527
2437.490748	34492.037748	58.668532
2436.612586	34255.754802	58.673537
2436.314184	34030.252872	58.678541
2435.442904	33797.305127	58.683546
2434.901025	33583.915166	58.688551
2434.015158	33357.466191	58.693556
2433.086075	33132.770184	58.698561
2432.844038	32914.990858	58.703565
2431.935338	32691.296322	58.708570
2431.133810	32469.566222	58.713575
2430.205639	32252.275755	58.718580
2429.375873	32032.736639	58.723585
2429.056408	31814.195611	58.728589
2428.182480	31605.973426	58.733594
2427.354296	31394.684416	58.738599
2426.592006	31178.538448	58.743604
2425.503478	30989.334721	58.748609
2425.079557	30769.130336	58.753613
2424.454015	30574.496960	58.758618
2423.249069	30378.023852	58.763623
2422.417120	30188.117207	58.768628
2421.462233	29998.298619	58.773633
2420.575549	29808.247074	58.778637
2419.554806	29633.262971	58.783642
2418.699025	29449.517741	58.788647
2418.159020	29281.535989	58.793652
2416.780346	29128.465448	58.798657
2415.916183	28968.072725	58.803661
2415.001375	28822.571694	58.808666
2413.883826	28673.134012	58.813671
2413.425580	28528.754415	58.818676
2412.311868	28392.892446	58.823681
2411.352370	28245.174586	58.828685
2410.435365	28141.790768	58.833690
2409.873244	28006.130527	58.838695
2408.932664	27881.006733	58.843700
2407.864571	27774.170616	58.848705
2407.171486	27657.037541	58.853709
2406.248103	27549.620743	58.858714
2405.311190	27456.466018	58.863719
2404.714448	27366.427558	58.868724
2403.426506	27271.647180	58.873729
2402.779796	27172.996577	58.878733
2402.338095	27097.325915	58.883738
2401.140423	27009.489642	58.888743
2400.681130	26931.120537	58.893748
2399.617651	26862.376046	58.898753
2399.117762	26776.185399	58.903757
2398.453996	26706.533880	58.908762
2397.554559	26622.276903	58.913767
2397.147022	26555.465858	58.918772
2396.293054	26479.791595	58.923777
2395.845445	26410.608612	58.928781
2395.036758	26341.924676	58.933786
2394.339575	26277.338187	58.938791
2393.958452	26204.877376	58.943796
2393.027888	26142.843920	58.948801
2392.603368	26074.927124	58.953805
2392.181282	26003.324316	58.958810
2391.559475	25941.365101	58.963815
2391.016179	25868.520837	58.968820
2390.232325	25795.989098	58.973825
2389.733286	25720.437472	58.978829
2389.388996	25647.161458	58.983834
2388.771480	25571.226541	58.988839
2388.511001	25497.771281	58.993844
2387.693947	25420.598788	58.998849
2387.173909	25335.027185	59.003853
2386.445921	25267.209315	59.008858
2385.823296	25189.668307	59.013863
2385.335931	25098.953938	59.018868
2384.826009	25024.930723	59.023873
2384.182039	24937.269153	59.028877
2383.059377	24859.088014	59.033882
2382.316522	24787.597577	59.038887
2382.085886	24706.424849	59.043892
2381.201310	24623.563573	59.048897
2380.637660	24549.148331	59.053901
2380.215374	24466.667862	59.058906
2379.317492	24385.248781	59.063911
2378.787117	24314.769970	59.068916
2377.919970	24235.516873	59.073921
2377.630494	24150.445737	59.078925
2376.930851	24076.614946	59.083930
2376.117343	23996.680141	59.088935
2375.633411	23920.186228	59.093940
2374.794341	23849.015342	59.098945
2374.066273	23765.186899	59.103949
2373.346535	23688.106865	59.108954
2372.727707	23608.659585	59.113959
2372.272480	23533.037932	59.118964
2371.471981	23455.922872	59.123969
2371.073370	23373.222425	59.128973
2370.430936	23298.330417	59.133978
2369.629525	23225.113538	59.138983
2369.713934	23129.438142	59.143988
2368.609148	23059.963277	59.148993
2368.121837	22964.277671	59.153997
2367.645335	22883.445393	59.159002
2366.552958	22803.939841	59.164007
2365.965098	22728.211190	59.169012
2364.931371	22651.045437	59.174017
2364.305754	22558.216568	59.179021
2363.900008	22490.109146	59.184026
2362.922631	22421.893681	59.189031
2362.392349	22330.147795	59.194036
2361.799213	22261.193829	59.199041
2360.981710	22181.839695	59.204045
2360.308358	22098.291706	59.209050
2360.031337	22031.264167	59.214055
2359.187002	21944.494964	59.219060
2358.160468	21876.497314	59.224065
2357.690896	21797.089944	59.229069
2357.071564	21727.267619	59.234074
2356.577977	21656.774272	59.239079
2356.245596	21582.463408	59.244084
2355.074428	21504.456544	59.249089
2354.233927	21430.662807	59.254093
2353.766540	21352.962768	59.259098
2353.229074	21279.031681	59.264103
2352.521264	21197.173303	59.269108
2351.785416	21131.574048	59.274113
2351.654357	21047.625875	59.279117
2350.866328	20968.676241	59.284122
2350.066433	20895.223606	59.289127
2349.360536	20813.615624	59.294132
2348.818130	20745.949150	59.299137
2348.070027	20660.235652	59.304141
2347.425778	20587.648376	59.309146
2346.750974	20511.407302	59.314151
2346.174899	20429.829680	59.319156
2345.378841	20368.715709	59.324161
2344.894491	20279.928411	59.329165
2344.398806	20201.447876	59.334170
2343.384624	20131.148933	59.339175
2342.571847	20046.688547	59.344180
2341.847644	19970.402678	59.349185
2341.004926	19901.349829	59.354189
2340.512028	19815.547589	59.359194
2339.856040	19752.066317	59.364199
2339.271034	19685.316703	59.369204
2338.804365	19617.232179	59.374209
2338.097609	19540.768405	59.379213
2337.032178	19457.031788	59.384218
2336.740958	19399.114241	59.389223
2336.284838	19325.050003	59.394228
2335.601362	19250.799942	59.399233
2335.057256	19167.693496	59.404237
2334.182143	19100.337549	59.409242
2333.483615	19023.310166	59.414247
2333.180488	18938.490758	59.419252
2332.197459	18877.944351	59.424257
2331.440547	18793.239142	59.429261
2331.055180	18716.275713	59.434266
2330.223662	18637.853531	59.439271
2329.680104	18561.445256	59.444276
2328.728743	18496.661705	59.449281
2328.081674	18422.255888	59.454285
2327.240577	18345.265128	59.459290
2326.615585	18278.628137	59.464295
2326.358670	18199.987975	59.469300
2325.021027	18140.497289	59.474305
2324.587609	18074.557821	59.479309
2324.093627	18001.114503	59.484314
2323.596133	17929.249662	59.489319
2323.199299	17854.713735	59.494324
2322.318890	17788.013580	59.499329
2321.723314	17703.065141	59.504333
2320.873921	17634.962167	59.509338
2319.973833	17563.765348	59.514343
2319.367873	17483.953557	59.519348
2319.007763	17424.969909	59.524353
2318.276232	17366.235226	59.529357
2317.948116	17283.753054	59.534362
2317.018527	17206.090520	59.539367
2316.514547	17136.604330	59.544372
2315.647199	17072.034826	59.549377
2315.005224	16978.774780	59.554381
2314.380323	16913.340470	59.559386
2313.424143	16842.919739	59.564391
2312.873336	16771.362948	59.569396
2312.068099	16701.371402	59.574401
2311.358974	16644.332942	59.579405
2310.969488	16567.465090	59.584410
2310.226252	16497.192722	59.589415
2309.638739	16430.082191	59.594420
2308.849784	16372.283488	59.599425
2308.093086	16295.583954	59.604429
2307.361786	16228.478162	59.609434
2306.565381	16157.642158	59.614439
2306.040421	16100.656419	59.619444
2305.449663	16041.613013	59.624449
2304.866825	15963.081883	59.629453
2304.176481	15894.502798	59.634458
2303.666509	15827.931634	59.639463
2303.146199	15760.797183	59.644468
2302.645526	15684.512045	59.649473
2301.837434	15612.702111	59.654477
2301.082580	15548.877760	59.659482
2300.227053	15480.912741	59.664487
2299.835219	15400.165792	59.669492
2298.805320	15343.599950	59.674497
2297.947580	15275.265446	59.679501
2297.556600	15208.216980	59.684506
2296.808936	15151.015653	59.689511
2296.232675	15081.308692	59.694516
2295.217951	15023.640548	59.699521
2294.886216	14953.605641	59.704525
2294.450596	14883.050660	59.709530
2293.798136	14820.200150	59.714535
2293.747220	14744.154670	59.719540
2292.925199	14671.062864	59.724545
2292.107850	14588.403496	59.729549
2291.188603	14512.209711	59.734554
2290.554067	14451.565644	59.739559
2290.029679	14381.329218	59.744564
2289.110170	14314.293910	59.749569
2288.475713	14237.940806	59.754573
2287.887662	14171.174954	59.759578
2286.829427	14113.368682	59.764583
2286.402483	14043.442215	59.769588
2285.938215	13972.647656	59.774593
2285.144624	13910.858642	59.779597
2284.370852	13840.893212	59.784602
2283.865117	13778.637170	59.789607
2283.029009	13695.777467	59.794612
2282.222956	13636.669166	59.799617
2281.820906	13578.982308	59.804621
2281.393198	13498.380501	59.809626
2280.565905	13432.774348	59.814631
2279.920267	13361.567519	59.819636
2279.097552	13303.393359	59.824641
2278.821856	13237.772175	59.829645
2277.516144	13172.451160	59.834650
2277.200960	13114.862268	59.839655
2276.821013	13039.313647	59.844660
2276.008244	12973.589000	59.849665
2275.178674	12900.873919	59.854669
2274.825946	12831.527064	59.859674
2273.893507	12773.010528	59.864679
2273.463503	12708.415120	59.869684
2273.102089	12634.136039	59.874689
2272.075327	12559.406928	59.879693
2271.415830	12479.308906	59.884698
2270.418473	12411.847008	59.889703
2270.166160	12347.650075	59.894708
2269.120221	12290.153185	59.899713
2268.556317	12218.767911	59.904718
2268.540334	12148.486200	59.909722
2267.537739	12087.745603	59.914727
2266.779828	12023.243391	59.919732
2266.100899	11948.290106	59.924737
2265.334140	11875.987792	59.929742
2264.873653	11813.314320	59.934746
2263.821520	11745.297533	59.939751
2263.252144	11667.260794	59.944756
2262.361111	11611.661689	59.949761
2261.752097	11541.895246	59.954766
2261.395443	11477.308244	59.959770
2260.653342	11416.364120	59.964775
2260.001873	11347.283491	59.969780
2259.131641	11304.508851	59.974785
2258.811606	11228.757752	59.979790
2258.076182	11152.726930	59.984794
2257.320825	11094.423342	59.989799
2256.891036	11020.852626	59.994804
2256.131402	10970.911665	59.999809
2255.225710	10897.660053	60.004814
2254.977373	10818.752254	60.009818
2254.010280	10763.661474	60.014823
2253.148474	10707.556103	60.019828
2252.670377	10625.454384	60.024833
2252.253662	10562.676194	60.029838
2251.567884	10497.596050	60.034842
2250.343310	10425.814349	60.039847
2250.188761	10387.029188	60.044852
2249.585942	10305.469729	60.049857
2248.829919	10237.642376	60.054862
2248.324995	10171.879706	60.059866
2247.521860	10103.062376	60.064871
2246.882888	10039.485704	60.069876
2246.212137	9984.751573	60.074881
2245.952814	9913.159657	60.079886
2245.097845	9845.529259	60.084890
2244.136697	9773.429996	60.089895
2243.538399	9692.553226	60.094900
2242.424221	9638.314757	60.099905
2241.888128	9583.625819	60.104910
2241.582292	9510.142628	60.109914
2240.765527	9455.802419	60.114919
2239.956001	9389.253242	60.119924
2239.248529	9329.064730	60.124929
2238.732884	9266.500148	60.129934
2238.227043	9207.803171	60.134938
2237.093388	9146.329591	60.139943
2237.041459	9068.763078	60.144948
2236.511439	9032.361581	60.149953
2235.635226	8952.713896	60.154958
2235.367148	8880.695575	60.159962
2234.447099	8826.299879	60.164967
2233.728154	8740.489102	60.169972
2233.183398	8676.520650	60.174977
2232.262928	8619.041573	60.179982
2231.562362	8556.564909	60.184986
2230.860371	8483.149988	60.189991
2230.074936	8403.279016	60.194996
2229.536319	8353.741266	60.200001
2228.584602	8314.945913	60.205006
2228.262329	8225.866400	60.210010
2227.524449	8181.277895	60.215015
2227.194765	8094.696335	60.220020
2226.288796	8063.349982	60.225025
2225.650715	7973.629444	60.230030
2225.367057	7927.124499	60.235034
2224.390102	7834.902643	60.240039
2223.778879	7794.341638	60.245044
2223.042897	7707.612206	60.250049
2222.264157	7645.120997	60.255054
2221.674709	7599.033185	60.260058
2220.973002	7536.501025	60.265063
2220.112035	7441.401300	60.270068
2219.768035	7404.617323	60.275073
2219.077569	7353.144374	60.280078
2218.639769	7278.813934	60.285082
2217.547298	7218.208306	60.290087
2217.299127	7141.670532	60.295092
2216.674284	7075.632075	60.300097
2215.728238	7022.769115	60.305102
2215.211065	6956.428559	60.310106
2214.347533	6891.476323	60.315111
2213.829255	6816.836761	60.320116
2212.680735	6778.831527	60.325121
2212.099454	6700.473103	60.330126
2211.842039	6641.079899	60.335130
2210.958491	6584.654293	60.340135
2210.311908	6514.173016	60.345140
2209.716015	6457.970449	60.350145
2209.521325	6395.871430	60.355150
2208.637371	6322.619089	60.360154
2208.032406	6262.084386	60.365159
2207.206558	6200.616362	60.370164
2206.632825	6130.821835	60.375169
2205.834722	6066.006396	60.380174
2205.002138	5994.803830	60.385178
2204.083254	5940.837745	60.390183
2203.861262	5877.702496	60.395188
2203.140220	5812.802589	60.400193
2202.350232	5756.931622	60.405198
2201.656240	5694.723873	60.410202
2201.007738	5640.943939	60.415207
2200.515401	5569.502517	60.420212
2200.022902	5514.527025	60.425217
2199.042355	5452.991217	60.430222
2198.716490	5393.807902	60.435226
2197.655135	5334.339251	60.440231
2197.325112	5264.618997	60.445236
2196.512335	5210.895874	60.450241
2195.635666	5147.324964	60.455246
2195.261784	5080.444805	60.460250
2194.564973	5025.059505	60.465255
2193.998513	4957.432790	60.470260
2193.134083	4890.937327	60.475265
2192.488193	4831.394546	60.480270
2192.383171	4771.950759	60.485274
2191.064345	4714.082339	60.490279
2190.445274	4636.374958	60.495284
2189.919600	4576.835431	60.500289
2188.959125	4523.051497	60.505294
2188.624280	4463.169840	60.510298
2187.987294	4418.862176	60.515303
2187.146250	4338.824772	60.520308
2186.496466	4290.217337	60.525313
2185.898883	4218.032579	60.530318
2185.474599	4144.611670	60.535322
2184.280439	4088.811944	60.540327
2184.046922	4043.196908	60.545332
2183.380627	3977.219895	60.550337
2182.725305	3913.955960	60.555342
2182.065844	3851.980019	60.560346
2181.252098	3796.128157	60.565351
2180.651223	3738.948584	60.570356
2179.824698	3671.911623	60.575361
2178.937753	3613.478256	60.580366
2178.472142	3549.075408	60.585370
2177.667860	3508.229929	60.590375
2177.176346	3438.798673	60.595380
2176.743495	3396.490048	60.600385
2176.034353	3326.264225	60.605390
2175.313336	3268.422609	60.610394
2174.371702	3221.178848	60.615399
2174.021028	3153.534094	60.620404
2173.573548	3092.870732	60.625409
2172.419721	3040.359448	60.630414
2172.058695	2974.687873	60.635418
2171.234378	2918.110013	60.640423
2170.628099	2856.716563	60.645428
2169.686037	2798.946572	60.650433
2168.918553	2741.716894	60.655438
2168.425005	2688.516998	60.660442
2167.612631	2630.092295	60.665447
2166.841618	2572.615438	60.670452
2166.408434	2536.477584	60.675457
2165.357853	2478.542343	60.680462
2165.612394	2412.526446	60.685466
2164.644867	2375.934385	60.690471
2164.097481	2316.402760	60.695476
2163.512835	2254.088164	60.700481
2162.769249	2194.379197	60.705486
2162.354886	2129.745791	60.710490
2161.806062	2081.138358	60.715495
2160.825269	2007.318099	60.720500
2160.217247	1952.382175	60.725505
2159.129158	1903.337301	60.730510
2158.583146	1843.007815	60.735514
2157.711944	1780.273108	60.740519
2157.252201	1722.687141	60.745524
2156.456796	1682.931177	60.750529
2155.320105	1631.496237	60.755534
2155.112192	1583.339459	60.760538
2154.489958	1536.883961	60.765543
2153.903954	1474.822877	60.770548
2153.088904	1428.694798	60.775553
2152.486843	1378.502212	60.780558
2152.058614	1324.951568	60.785562
2151.062634	1274.252537	60.790567
2150.516864	1214.856056	60.795572
2149.788603	1168.206453	60.800577
2149.261604	1110.931633	60.805582
2148.387838	1057.164075	60.810586
2147.459413	1020.750586	60.815591
2147.252005	955.014065	60.820596
2146.354224	910.842015	60.825601
2145.538489	860.212033	60.830606
2144.992226	812.821125	60.835610
2144.430499	773.276590	60.840615
2143.808690	713.783838	60.845620
2143.169165	669.915325	60.850625
2142.252177	618.721938	60.855630
2141.529675	574.639800	60.860634
2140.545857	521.219696	60.865639
2139.927504	468.989150	60.870644
2139.328167	434.089235	60.875649
2138.493071	401.013451	60.880654
2137.931228	339.241971	60.885658
2137.070045	328.871655	60.890663
2136.790232	281.839168	60.895668
2135.928665	240.263734	60.900673
2135.004214	202.325246	60.905678
2134.534225	166.623317	60.910682
2133.289302	127.334021	60.915687
2133.195342	102.347438	60.920692
2132.544825	65.234711	60.925697
2131.527333	37.999493	60.930702
2130.963038	4.927384	60.935706
2129.871892	-30.396397	60.940711
2128.733398	-49.455118	60.945716
2122.634466	76.487437	60.950721
2121.638412	107.896044	60.955726
2123.215262	106.791155	60.960730
2124.379845	110.669972	60.965735
2125.107466	108.930309	60.970740
2125.058307	103.354347	60.975745
2124.056790	103.115851	60.980750
2123.310530	90.813146	60.985754
2121.668095	109.723479	60.990759
2121.254646	101.262858	60.995764
2120.579048	100.367129	61.000769
2119.380934	108.167228	61.005774
2119.239999	116.343617	61.010778
2118.617092	107.318588	61.015783
2118.022016	102.261311	61.020788
2117.473566	98.876015	61.025793
2116.370415	110.576442	61.030798
2116.442905	101.472619	61.035802
2115.669429	109.894440	61.040807
2115.195045	103.395667	61.045812
2114.180687	101.523988	61.050817
2113.252195	106.081818	61.055822
2112.504565	94.071055	61.060826
2111.604620	112.743743	61.065831
2111.900116	106.734642	61.070836
2111.554348	109.224182	61.075841
2110.560371	102.068296	61.080846
2110.012676	112.543662	61.085850
2109.132890	117.527411	61.090855
2108.260945	105.027034	61.095860
2107.771642	104.962725	61.100865
2106.683537	111.431834	61.105870
2105.816371	114.155487	61.110874
2105.304891	119.654783	61.115879
2105.684358	109.195011	61.120884
2104.409996	112.405879	61.125889
2103.444984	110.059616	61.130894
2103.487646	108.739277	61.135898
2102.695057	111.320216	61.140903
2101.968401	111.247841	61.145908
2101.304596	106.958375	61.150913
2100.472131	112.628444	61.155918
2099.971656	105.222376	61.160922
2099.005318	114.281904	61.165927
2098.292037	108.308296	61.170932
2097.675717	102.532184	61.175937
2096.766566	112.230735	61.180942
2096.447547	89.829713	61.185946
2096.527612	106.632825	61.190951
2095.344687	107.927469	61.195956
2094.465329	106.165257	61.200961
2094.081194	108.883226	61.205966
2093.320518	107.442788	61.210970
2093.216552	105.144398	61.215975
2091.835767	104.597105	61.220980
2091.250744	111.279691	61.225985
2090.671864	104.917347	61.230990
2090.699788	102.238501	61.235994
2088.845406	110.013443	61.240999
2088.926669	110.035212	61.246004
2088.213006	102.847472	61.251009
2087.046440	111.870968	61.256014
2087.016201	105.071500	61.261018
2086.593230	106.830582	61.266023
2085.073687	111.568938	61.271028
2084.648340	117.557593	61.276033
2084.332244	110.715177	61.281038
2083.605118	109.627370	61.286042
2082.539721	108.143829	61.291047
2082.145955	108.051751	61.296052
2081.919300	104.684782	61.301057
2080.530775	117.277293	61.306062
2080.398184	104.765258	61.311066
2079.338098	112.721659	61.316071
2079.143440	109.491531	61.321076
2077.853604	114.068868	61.326081
2077.794978	108.527524	61.331086
2077.269854	112.414260	61.336090
2075.811402	114.484307	61.341095
2075.536336	104.085826	61.346100
2075.301216	110.444821	61.351105
2073.746110	118.143903	61.356110
2074.039452	96.583951	61.361114
2072.749566	123.742225	61.366119
2071.984372	111.246996	61.371124
2071.952911	97.580413	61.376129
2070.958893	113.964216	61.381134
2070.094403	111.089528	61.386138
2069.989805	106.034852	61.391143
2068.851413	98.145002	61.396148
2067.675105	102.224953	61.401153
2067.940488	111.169452	61.406158
2067.843117	102.644494	61.411162
2066.495360	106.642849	61.416167
2065.496330	110.112803	61.421172
2064.552176	109.590850	61.426177
2063.878337	115.160066	61.431182
2064.107488	114.803569	61.436186
2063.071379	115.278605	61.441191
2062.383806	113.003443	61.446196
2061.736737	112.923180	61.451201
2061.075409	111.396027	61.456206
2060.506488	103.841567	61.461210
2059.978551	99.622014	61.466215
2059.195251	105.940270	61.471220
2058.667881	112.087034	61.476225
2057.838493	108.484570	61.481230
2057.523261	107.902238	61.486234
2056.855071	112.439279	61.491239
2056.366320	114.921555	61.496244
2055.614341	106.839506	61.501249
2053.694296	113.223045	61.506254
2053.970124	108.169498	61.511258
2053.395607	119.106425	61.516263
2052.575955	110.768621	61.521268
2051.639309	94.014664	61.526273
2050.743927	111.330518	61.531278
2050.973221	108.856247	61.536282
2049.790831	102.435154	61.541287
2048.861337	113.505678	61.546292
2048.798271	101.625985	61.551297
2047.834278	107.651236	61.556302
2047.725564	111.973343	61.561306
2046.955252	118.653806	61.566311
2046.511424	117.921579	61.571316
2046.035994	104.634518	61.576321
2044.895220	100.644680	61.581326
2043.768614	103.863662	61.586330
2043.098219	106.854136	61.591335
2042.150151	114.355977	61.596340
2042.350263	102.491287	61.601345
2041.290612	105.852603	61.606350
2040.662414	101.002445	61.611354
2039.931108	114.684368	61.616359
2039.231477	117.140191	61.621364
2039.112553	100.803640	61.626369
2038.136551	107.054717	61.631374
2037.991080	101.036751	61.636378
2037.000173	105.585586	61.641383
2036.452383	114.134029	61.646388
2035.564953	108.328421	61.651393
2034.254834	115.572346	61.656398
2033.847008	103.342109	61.661402
2033.242626	106.068231	61.666407
2033.140868	106.721412	61.671412
2032.586496	103.458495	61.676417
2031.500203	113.653508	61.681422
2030.887743	111.812693	61.686426
2030.353388	111.878545	61.691431
2029.946833	118.920733	61.696436
2029.431370	95.352474	61.701441
2027.994587	118.907241	61.706446
2027.440358	116.705540	61.711450
2026.771424	111.991151	61.716455
2025.775450	114.366280	61.721460
2025.632884	122.032017	61.726465
2024.402346	127.828361	61.731470
2024.408182	111.249662	61.736474
2023.941696	110.689762	61.741479
2023.288051	113.985074	61.746484
2023.051234	113.074926	61.751489
2021.702193	119.658014	61.756494
2020.798310	117.740454	61.761498
2020.040983	112.440881	61.766503
2019.023981	116.844063	61.771508
2019.107396	116.037627	61.776513
2018.534085	118.503368	61.781518
2017.713201	105.485596	61.786522
2017.197080	107.899684	61.791527
2016.850617	117.395421	61.796532
2016.294212	107.341208	61.801537
2014.962518	117.016960	61.806542
2014.204407	111.083608	61.811546
2013.462659	109.641767	61.816551
2012.696440	111.644561	61.821556
2012.574753	104.515853	61.826561
2011.956791	103.037022	61.831566
2011.366244	108.613527	61.836570
2011.254322	114.721171	61.841575
2010.299451	113.538648	61.846580
2009.126958	96.371154	61.851585
2008.063257	110.602548	61.856590
2007.728262	102.755525	61.861594
2007.251347	101.883484	61.866599
2006.312588	110.590168	61.871604
2006.106461	95.612548	61.876609
2005.417848	111.525287	61.881614
2004.504476	106.077030	61.886618
2003.765761	107.591359	61.891623
2002.456864	112.800928	61.896628
2002.310613	105.529470	61.901633
2001.622164	114.991177	61.906638
2001.114229	105.714564	61.911642
2000.638538	109.874151	61.916647
1999.957929	108.091466	61.921652
1999.890965	109.007195	61.926657
1999.297646	117.613330	61.931662
1998.294054	118.116344	61.936666
1997.206775	111.511453	61.941671
1996.470347	121.452267	61.946676
1996.377423	106.891891	61.951681
1995.366187	100.322243	61.956686
1994.735638	106.193667	61.961690
1993.543483	117.145052	61.966695
1992.655919	115.064070	61.971700
1993.067042	99.794527	61.976705
1991.938958	112.722606	61.981710
1991.610425	100.125002	61.986714
1991.291912	97.884324	61.991719
1990.351231	105.922718	61.996724
1989.483682	109.048569	62.001729
1988.230947	112.822156	62.006734
1987.511249	105.581793	62.011738
1987.252807	103.270082	62.016743
1986.299813	112.565630	62.021748
1986.207389	107.846482	62.026753
1985.844804	107.002028	62.031758
1985.422198	103.054344	62.036762
1984.425873	106.397744	62.041767
1983.135580	114.206219	62.046772
1982.735165	114.640312	62.051777
1981.747616	110.320267	62.056782
1981.390528	106.146151	62.061786
1981.173596	103.239677	62.066791
1980.276988	108.749652	62.071796
1980.045381	109.395060	62.076801
1978.858234	117.926724	62.081806
1977.732882	108.199358	62.086810
1977.274680	101.548248	62.091815
1976.642677	113.479851	62.096820
1976.315041	98.332297	62.101825
1976.004776	111.048577	62.106830
1975.273877	104.680434	62.111834
1974.475134	103.337534	62.116839
1973.191370	108.861655	62.121844
1972.839645	106.560020	62.126849
1972.087431	106.978993	62.131854
1971.864816	99.626627	62.136858
1971.327058	100.200786	62.141863
1970.042947	111.900018	62.146868
1969.393267	100.219099	62.151873
1968.596363	104.235716	62.156878
1968.286853	105.868001	62.161882
1968.038630	102.449279	62.166887
1967.454833	109.904358	62.171892
1966.569363	109.879304	62.176897
1965.502650	106.733992	62.181902
1964.482002	106.662589	62.186906
1964.275850	110.501867	62.191911
1963.642665	106.874602	62.196916
1963.194940	99.986879	62.201921
1962.715038	107.603653	62.206926
1961.697480	104.127281	62.211930
1961.010008	111.780159	62.216935
1959.828180	114.359844	62.221940
1959.706417	106.171492	62.226945
1958.993974	112.442258	62.231950
1958.572946	102.489576	62.236954
1958.167995	105.540432	62.241959
1957.002851	117.124600	62.246964
1956.129259	102.937296	62.251969
1955.351718	112.597645	62.256974
1955.098564	117.931383	62.261978
1954.668967	106.657058	62.266983
1954.088819	103.062376	62.271988
1953.891710	103.185095	62.276993
1952.538062	105.907167	62.281998
1951.582458	111.412323	62.287002
1950.945371	108.801190	62.292007
1950.234232	109.428104	62.297012
1950.334287	107.631900	62.302017
1948.847694	111.962993	62.307022
1948.150670	111.766114	62.312026
1947.572740	107.341643	62.317031
1946.752968	110.076742	62.322036
1946.790066	109.022202	62.327041
1946.215064	111.999133	62.332046
1945.682367	111.279454	62.337050
1944.875767	102.166956	62.342055
1943.570674	116.752064	62.347060
1943.257216	105.147086	62.352065
1942.909798	113.244283	62.357070
1942.082620	110.429948	62.362074
1941.017769	102.872247	62.367079
1939.859455	106.810629	62.372084
1939.974079	106.588990	62.377089
1938.980291	117.154107	62.382094
1938.470133	110.965391	62.387098
1938.261488	109.921475	62.392103
1937.427274	115.940354	62.397108
1937.342926	100.279550	62.402113
1935.941734	116.128801	62.407118
1935.092254	107.942430	62.412122
1934.742107	105.883391	62.417127
1934.266992	107.636579	62.422132
1933.380606	106.198799	62.427137
1932.349376	110.060244	62.432142
1931.713519	113.810047	62.437146
1931.064191	107.468392	62.442151
1930.481262	117.572497	62.447156
1930.393172	106.341736	62.452161
1929.686525	107.166629	62.457166
1929.239967	107.388867	62.462170
1928.098823	110.359480	62.467175
1927.086812	116.909609	62.472180
1926.836929	100.552874	62.477185
1925.976638	113.810606	62.482190
1925.678669	103.699632	62.487194
1924.788183	98.594691	62.492199
1923.609679	102.195678	62.497204
1922.988660	99.709731	62.502209
1922.790786	105.414717	62.507214
1922.222191	99.454472	62.512218
1922.004633	96.387265	62.517223
1920.928857	100.632656	62.522228
1919.892274	104.647911	62.527233
1919.186567	106.617470	62.532238
1918.542531	103.550156	62.537242
1918.452444	99.715273	62.542247
1917.609273	108.898790	62.547252
1917.423307	113.381386	62.552257
1915.802422	102.578445	62.557262
1915.162696	112.302076	62.562266
1914.742450	115.058914	62.567271
1914.345977	111.055056	62.572276
1913.991939	104.387425	62.577281
1912.875748	109.575902	62.582286
1911.732587	110.821738	62.587290
1911.602058	107.264497	62.592295
1910.602116	107.532010	62.597300
1910.493553	99.953401	62.602305
1909.924063	110.362860	62.607310
1909.244071	106.437126	62.612314
1908.204100	109.489453	62.617319
1907.244365	111.122468	62.622324
1907.228366	104.599862	62.627329
1906.624391	116.859748	62.632334
1905.373266	108.715072	62.637338
1904.666141	102.360527	62.642343
1903.908548	110.853983	62.647348
1903.467771	106.797240	62.652353
1902.875889	105.115610	62.657358
1902.343600	105.267888	62.662362
1902.106137	105.641432	62.667367
1901.065938	105.383932	62.672372
1900.513520	102.432959	62.677377
1899.892818	111.445554	62.682382
1899.133852	110.853263	62.687386
1898.948733	98.526217	62.692391
1897.552622	112.849832	62.697396
1896.720997	104.102431	62.702401
1896.075112	103.992060	62.707406
1895.742954	107.189055	62.712410
1895.286121	106.958790	62.717415
1894.559942	120.837033	62.722420
1893.836668	106.044026	62.727425
1893.045097	110.709491	62.732430
1892.468619	105.671400	62.737434
1892.037541	106.269637	62.742439
1890.931503	114.384773	62.747444
1890.351201	107.062394	62.752449
1889.525750	96.494304	62.757454
1888.865236	109.884319	62.762458
1888.668406	97.896587	62.767463
1888.172548	108.906186	62.772468
1887.426721	101.570666	62.777473
1886.263936	118.545824	62.782478
1885.868196	109.196240	62.787482
1885.234602	101.740406	62.792487
1884.645441	114.098859	62.797492
1883.681097	100.550444	62.802497
1882.641648	118.655565	62.807502
1882.301164	98.416763	62.812506
1881.473656	111.576261	62.817511
1881.032638	118.571895	62.822516
1880.770489	97.899631	62.827521
1880.562894	112.198562	62.832526
1879.531859	110.741189	62.837530
1878.628142	101.229418	62.842535
1877.849312	113.480795	62.847540
1877.374041	107.668162	62.852545
1876.462801	99.617775	62.857550
1875.377065	103.295513	62.862554
1874.933382	101.287602	62.867559
1874.241345	109.021639	62.872564
1874.194830	100.822931	62.877569
1873.838149	107.026194	62.882574
1873.118907	101.843626	62.887578
1872.215747	92.174088	62.892583
1871.556130	110.548466	62.897588
1871.019295	97.230219	62.902593
1869.677775	105.797461	62.907598
1868.614969	105.303877	62.912602
1868.140734	105.435908	62.917607
1867.296037	104.313216	62.922612
1867.307113	105.938766	62.927617
1867.084297	107.856904	62.932622
1866.452444	91.045200	62.937626
1865.798095	113.302588	62.942631
1864.804970	85.685145	62.947636
1863.782389	102.086124	62.952641
1863.380658	110.622433	62.957646
1862.981717	100.620542	62.962650
1862.390029	96.411160	62.967655
1861.174661	103.756797	62.972660
1860.468107	103.717565	62.977665
1860.130495	102.859704	62.982670
1859.568495	107.201737	62.987674
1858.976337	102.481521	62.992679
1857.683520	106.499634	62.997684
1857.573858	112.471303	63.002689
1856.812963	105.811511	63.007694
1856.720260	109.112412	63.012698
1855.568842	99.909625	63.017703
1854.417737	106.423510	63.022708
1853.813709	104.165107	63.027713
1853.478172	100.809146	63.032718
1852.672402	109.283453	63.037722
1852.546690	100.378267	63.042727
1851.445662	110.080532	63.047732
1850.866095	101.890768	63.052737
1850.188790	102.412993	63.057742
1849.918088	108.479611	63.062746
1849.265021	105.262369	63.067751
1847.569286	106.389392	63.072756
1847.156496	101.883540	63.077761
1846.792361	96.460108	63.082766
1846.449338	98.249105	63.087770
1846.069996	100.313514	63.092775
1844.917345	108.664710	63.097780
1844.163462	88.996171	63.102785
1843.811772	100.815467	63.107790
1843.400955	97.070935	63.112794
1842.468103	95.966978	63.117799
1841.055191	103.607325	63.122804
1840.659598	102.317148	63.127809
1840.450751	101.177084	63.132814
1839.777722	105.872623	63.137818
1839.332713	99.821820	63.142823
1838.357562	103.742198	63.147828
1837.714131	97.205686	63.152833
1837.036026	95.924096	63.157838
1836.406803	95.244997	63.162842
1835.648620	88.381373	63.167847
1834.469499	108.347302	63.172852
1833.963388	89.757432	63.177857
1833.540216	101.042479	63.182862
1833.327971	103.821491	63.187866
1832.713076	106.344328	63.192871
1831.678050	106.486561	63.197876
1830.933483	99.562427	63.202881
1830.346958	98.931740	63.207886
1829.623088	100.476871	63.212890
1829.426212	102.997989	63.217895
1828.030207	105.124480	63.222900
1827.372834	94.277431	63.227905
1827.064808	99.102665	63.232910
1826.362755	101.212008	63.237914
1826.457127	96.075307	63.242919
1825.268194	97.427789	63.247924
1824.115348	94.509096	63.252929
1823.674676	96.893889	63.257934
1822.742068	104.327102	63.262938
1822.810677	96.540611	63.267943
1821.906749	104.697787	63.272948
1820.687596	88.441381	63.277953
1820.401659	97.146947	63.282958
1819.954600	88.696476	63.287962
1819.546635	100.644550	63.292967
1818.623467	109.367728	63.297972
1817.786309	103.491152	63.302977
1817.054919	103.462183	63.307982
1816.225846	105.878689	63.312986
1816.329135	95.929526	63.317991
1815.149392	107.747850	63.322996
1814.417793	103.702613	63.328001
1813.874506	95.518142	63.333006
1813.235923	97.357226	63.338010
1813.016200	94.093266	63.343015
1811.434179	108.957335	63.348020
1810.939512	101.148323	63.353025
1810.589720	95.907115	63.358030
1809.829706	105.714507	63.363034
1809.872673	91.359676	63.368039
1808.559922	101.999115	63.373044
1807.444788	99.998490	63.378049
1807.095745	93.636007	63.383054
1806.633191	104.373828	63.388058
1806.284328	100.851266	63.393063
1805.644438	100.990689	63.398068
1804.730197	90.726883	63.403073
1804.107900	95.321335	63.408078
1803.131154	96.427256	63.413082
1802.851817	94.563566	63.418087
1801.599353	99.795795	63.423092
1800.912873	96.538145	63.428097
1800.524148	99.941239	63.433102
1799.986988	96.860142	63.438106
1799.777611	93.503082	63.443111
1798.901905	108.259733	63.448116
1797.776892	102.682750	63.453121
1797.114417	96.048355	63.458126
1796.757634	104.561759	63.463130
1796.751758	88.324015	63.468135
1795.531443	103.395566	63.473140
1794.623422	97.490833	63.478145
1793.849830	98.766338	63.483150
1793.293784	107.546339	63.488154
1793.426535	91.497882	63.493159
1791.964565	96.460622	63.498164
1791.416692	100.330512	63.503169
1790.902105	99.797216	63.508174
1790.215565	98.576900	63.513178
1789.299702	93.409815	63.518183
1788.207023	97.422984	63.523188
1787.796883	99.739859	63.528193
1787.423565	102.866133	63.533198
1786.980486	107.205063	63.538202
1786.829210	89.235347	63.543207
1785.422921	96.387410	63.548212
1784.575858	88.402569	63.553217
1784.200590	95.118114	63.558222
1783.628386	97.339305	63.563226
1783.329516	88.434826	63.568231
1781.926457	100.074161	63.573236
1781.493678	94.429842	63.578241
1781.268722	85.488398	63.583246
1780.195287	92.155543	63.588250
1779.370999	86.404672	63.593255
1778.515317	98.374957	63.598260
1778.125517	98.525133	63.603265
1777.655775	105.369220	63.608270
1777.227006	95.534510	63.613274
1776.258342	86.540862	63.618279
1775.489350	104.631422	63.623284
1774.764382	102.668197	63.628289
1774.591248	83.634418	63.633294
1773.458167	103.012753	63.638298
1772.729480	89.286643	63.643303
1771.461739	98.791483	63.648308
1771.323169	92.070750	63.653313
1770.826652	89.144048	63.658318
1770.494251	95.017044	63.663322
1770.425464	94.504418	63.668327
1769.331866	98.885152	63.673332
1768.839198	93.870058	63.678337
1767.870829	92.601467	63.683342
1766.439253	101.662420	63.688346
1766.137293	89.412308	63.693351
1765.362423	105.919047	63.698356
1765.060991	102.201312	63.703361
1764.850597	97.354270	63.708366
1763.927715	99.965451	63.713370
1762.812619	100.306497	63.718375
1761.896624	101.830119	63.723380
1761.564805	96.903018	63.728385
1761.191718	95.431094	63.733390
1760.357875	108.057055	63.738394
1760.145371	98.334653	63.743399
1759.233244	98.998266	63.748404
1758.539885	92.174834	63.753409
1758.015581	80.428372	63.758414
1756.424313	94.685247	63.763418
1755.460610	93.939442	63.768423
1755.411123	100.259498	63.773428
1755.532171	86.969284	63.778433
1755.159886	90.524304	63.783438
1754.218224	103.030196	63.788442
1753.246238	96.202128	63.793447
1752.478736	91.080881	63.798452
1751.716863	105.418935	63.803457
1751.541785	94.350251	63.808462
1750.187525	97.815224	63.813466
1749.602780	93.131709	63.818471
1749.050059	99.000275	63.823476
1748.628145	101.918237	63.828481
1748.297090	95.261188	63.833486
1746.896369	94.556403	63.838490
1746.535881	95.815202	63.843495
1745.905684	100.953365	63.848500
1745.618273	86.624208	63.853505
1744.847064	94.022344	63.858510
1743.664915	96.084954	63.863514
1743.500677	87.261600	63.868519
1742.718812	89.060378	63.873524
1741.677097	94.740108	63.878529
1741.115951	88.550090	63.883534
1740.348976	96.409579	63.888538
1740.136920	89.164384	63.893543
1739.777639	98.569116	63.898548
1738.590618	89.425667	63.903553
1737.995967	89.876450	63.908558
1736.939915	94.949786	63.913562
1736.797125	91.566390	63.918567
1735.986802	100.481388	63.923572
1734.923375	100.585593	63.928577
1734.601010	95.732686	63.933582
1733.667461	100.504310	63.938586
1733.750649	96.679769	63.943591
1733.117309	96.717249	63.948596
1731.979443	93.383080	63.953601
1731.505000	94.524366	63.958606
1730.729027	94.958218	63.963610
1730.393029	93.989738	63.968615
1728.893945	95.867734	63.973620
1728.251374	99.979744	63.978625
1728.016175	102.959515	63.983630
1727.263482	94.882440	63.988634
1727.040289	95.838753	63.993639
1725.961304	97.859757	63.998644
1725.370802	90.862315	64.003649
1724.916050	89.556323	64.008654
1724.190964	100.599178	64.013658
1723.566247	100.692058	64.018663
1722.542715	97.686647	64.023668
1721.783709	94.245007	64.028673
1721.491002	107.910921	64.033678
1720.642319	99.235687	64.038682
1720.396295	82.580387	64.043687
1719.431969	90.611563	64.048692
1718.741583	90.771641	64.053697
1718.447043	92.303805	64.058702
1717.550092	95.869620	64.063706
1716.648276	87.543438	64.068711
1715.961501	95.308198	64.073716
1715.189383	84.435270	64.078721
1715.130967	98.708905	64.083726
1714.323622	98.947481	64.088730
1713.432122	93.049620	64.093735
1712.557449	89.017682	64.098740
1711.803221	92.094077	64.103745
1711.577028	95.767818	64.108750
1711.133349	92.049032	64.113754
1710.552684	96.971187	64.118759
1709.376020	97.996935	64.123764
1708.759020	84.633145	64.128769
1708.800635	84.101410	64.133774
1707.513564	92.680563	64.138778
1706.667753	80.403315	64.143783
1705.777890	95.099143	64.148788
1705.430415	87.367709	64.153793
1705.443448	90.979801	64.158798
1704.267900	95.351497	64.163802
1703.720204	96.360927	64.168807
1702.925094	95.564712	64.173812
1702.483635	90.388546	64.178817
1702.007522	86.752182	64.183822
1700.635394	98.741432	64.188826
1700.413125	91.523094	64.193831
1699.722243	96.927933	64.198836
1699.160307	95.298364	64.203841
1697.887262	97.053749	64.208846
1697.115997	98.093958	64.213850
1696.685601	88.614329	64.218855
1696.333560	99.645245	64.223860
1696.032576	94.852024	64.228865
1695.674237	94.295507	64.233870
1694.236957	96.944258	64.238874
1694.005451	87.578113	64.243879
1693.427330	88.751641	64.248884
1692.281767	95.080208	64.253889
1691.784227	93.505065	64.258894
1691.061652	99.135702	64.263898
1690.754455	97.557134	64.268903
1690.007325	100.001660	64.273908
1688.627691	95.572139	64.278913
1688.314744	93.390543	64.283918
1687.786387	86.944610	64.288922
1687.334201	88.773038	64.293927
1686.226774	87.736290	64.298932
1685.374282	94.478756	64.303937
1685.026182	90.257542	64.308942
1684.479718	102.565069	64.313946
1684.271893	92.146542	64.318951
1683.090531	99.379616	64.323956
1682.199700	97.742369	64.328961
1682.052640	84.754933	64.333966
1681.283608	104.915940	64.338970
1680.537648	91.369221	64.343975
1679.509133	97.009032	64.348980
1678.968252	99.025006	64.353985
1678.867705	101.332144	64.358990
1678.259569	103.953282	64.363994
1677.384870	94.698759	64.368999
1676.486561	90.774662	64.374004
1675.911068	98.018733	64.379009
1675.428070	96.871769	64.384014
1674.221016	110.206698	64.389018
1673.466404	102.368052	64.394023
1672.885069	101.703462	64.399028
1672.473289	96.448474	64.404033
1671.987713	91.768152	64.409038
1671.579211	103.921310	64.414042
1670.559486	92.613085	64.419047
1669.494025	102.142604	64.424052
1668.915206	102.661847	64.429057
1668.862665	95.629431	64.434062
1668.558731	100.988584	64.439066
1667.869657	97.053331	64.444071
1666.967678	95.053603	64.449076
1665.874807	99.547794	64.454081
1664.882053	105.850526	64.459086
1663.866260	99.844699	64.464090
1663.575504	96.439082	64.469095
1663.036825	95.832372	64.474100
1662.405760	88.555979	64.479105
1662.699702	95.308730	64.484110
1661.770695	108.832874	64.489114
1660.978903	103.989889	64.494119
1660.463069	90.532776	64.499124
1659.391512	93.878774	64.504129
1658.434786	85.432037	64.509134
1657.230851	106.688671	64.514138
1657.240735	80.889460	64.519143
1656.841389	86.068232	64.524148
1656.497972	99.094096	64.529153
1655.782313	92.032980	64.534158
1654.827913	95.633169	64.539162
1654.352032	94.376276	64.544167
1653.699697	97.639918	64.549172
1652.378797	92.992942	64.554177
1651.729654	86.463709	64.559182
1650.892872	95.195276	64.564186
1650.714091	107.332447	64.569191
1650.661581	97.778608	64.574196
1649.549238	92.201267	64.579201
1648.979368	118.431574	64.584206
1648.118116	96.536288	64.589210
1647.721224	112.328606	64.594215
1646.762829	95.346522	64.599220
1645.901207	103.236838	64.604225
1645.592573	97.773092	64.609230
1644.971216	95.169007	64.614234
1644.556938	100.036360	64.619239
1643.720928	90.886089	64.624244
1642.793928	101.557352	64.629249
1642.583497	103.883523	64.634254
1641.745345	96.132275	64.639258
1640.481747	84.984230	64.644263
1640.221788	98.983957	64.649268
1639.424318	97.959490	64.654273
1639.323817	101.482390	64.659278
1638.114827	104.549046	64.664282
1637.466701	95.335816	64.669287
1636.861407	97.027733	64.674292
1636.194797	99.675513	64.679297
1635.627693	100.670694	64.684302
1634.583564	103.749009	64.689306
1633.695538	92.736834	64.694311
1633.574680	87.348916	64.699316
1633.155286	96.290138	64.704321
1632.929274	87.452961	64.709326
1631.853279	101.569704	64.714330
1631.192510	91.675700	64.719335
1630.528908	89.808422	64.724340
1629.178222	97.696008	64.729345
1628.768871	90.198334	64.734350
1627.716249	101.875101	64.739354
1627.499280	98.609147	64.744359
1627.217377	103.026566	64.749364
1626.351714	97.960376	64.754369
1626.272259	95.080989	64.759374
1625.067183	101.706027	64.764378
1624.417604	92.302232	64.769383
1624.047347	98.275864	64.774388
1622.767656	97.465194	64.779393
1622.248789	94.411195	64.784398
1621.537779	99.830286	64.789402
1621.268461	97.622846	64.794407
1620.733493	92.881000	64.799412
1619.444538	101.182963	64.804417
1619.010644	85.566731	64.809422
1618.218335	91.192689	64.814426
1618.070566	86.841898	64.819431
1617.055063	97.684911	64.824436
1615.803882	100.364061	64.829441
1615.480570	95.498711	64.834446
1614.775379	95.259066	64.839450
1614.685720	96.668812	64.844455
1614.604605	97.555257	64.849460
1613.226735	105.243756	64.854465
1612.712250	89.392755	64.859470
1612.092798	95.305054	64.864474
1611.076529	96.191831	64.869479
1610.258596	93.500718	64.874484
1609.408712	100.092989	64.879489
1609.505762	96.898573	64.884494
1608.640768	101.545810	64.889498
1607.563269	101.447309	64.894503
1607.091622	94.640744	64.899508
1606.297130	99.948527	64.904513
1606.128095	90.569320	64.909518
1605.390918	94.141324	64.914522
1604.597257	95.098390	64.919527
1603.849483	97.347508	64.924532
1603.145454	99.783632	64.929537
1602.764029	91.086260	64.934542
1601.680194	97.551703	64.939546
1600.924745	89.091937	64.944551
1600.498435	92.508907	64.949556
1599.570355	98.415049	64.954561
1599.654461	94.945159	64.959566
1599.002478	95.575383	64.964570
1597.992618	98.697150	64.969575
1597.403889	90.453737	64.974580
1596.570181	99.984304	64.979585
1596.212394	98.355441	64.984590
1594.793108	97.019787	64.989594
1594.097619	95.282157	64.994599
1593.896810	101.771317	64.999604
1593.302446	94.638916	65.004609
1593.491862	87.498690	65.009614
1592.038204	96.672030	65.014618
1591.186041	98.188721	65.019623
1590.801546	87.359913	65.024628
1590.046563	88.842243	65.029633
1589.219324	90.500047	65.034638
1588.300668	99.629394	65.039642
1587.994409	96.350825	65.044647
1587.645388	92.653295	65.049652
1586.989756	98.274896	65.054657
1586.066601	83.188967	65.059662
1585.335564	84.449886	65.064666
1584.777613	88.657283	65.069671
1584.424247	84.101052	65.074676
1583.404865	98.082660	65.079681
1582.540546	92.634672	65.084686
1581.897736	110.538063	65.089690
1581.341970	110.213191	65.094695
1581.094735	93.294773	65.099700
1580.003895	91.995252	65.104705
1579.321614	87.123865	65.109710
1578.691299	95.433161	65.114714
1578.239654	93.246809	65.119719
1577.257055	92.551380	65.124724
1576.468450	91.678481	65.129729
1575.962266	86.436939	65.134734
1575.190585	113.339503	65.139738
1575.132465	97.430195	65.144743
1574.730024	98.955864	65.149748
1573.184682	92.707799	65.154753
1572.955700	88.521295	65.159758
1572.423624	103.898286	65.164762
1571.967547	94.794909	65.169767
1570.979098	88.125653	65.174772
1570.047806	102.919553	65.179777
1570.111491	88.137290	65.184782
1568.500555	111.800265	65.189786
1567.538705	92.191710	65.194791
1567.243529	84.609686	65.199796
1566.817115	90.822464	65.204801
1566.443603	80.843432	65.209806
1565.967318	85.621297	65.214810
1565.141411	92.307532	65.219815
1564.273001	94.471753	65.224820
1563.638349	92.688198	65.229825
1563.304847	82.333821	65.234830
1562.069727	89.968117	65.239834
1561.375978	87.082261	65.244839
1560.811584	96.226287	65.249844
1560.115047	96.953481	65.254849
1560.353051	79.464431	65.259854
1559.296760	99.335205	65.264858
1558.443978	90.916149	65.269863
1558.090903	90.987987	65.274868
1556.987685	96.918813	65.279873
1556.435125	90.022621	65.284878
1555.679545	92.689284	65.289882
1554.728605	93.940998	65.294887
1554.008424	83.968163	65.299892
1552.961957	96.476554	65.304897
1552.874147	94.522545	65.309902
1552.193238	99.571034	65.314906
1551.970235	100.659788	65.319911
1551.745317	91.611149	65.324916
1550.451487	94.596709	65.329921
1549.638481	89.325077	65.334926
1549.428636	94.076383	65.339930
1548.427383	93.390236	65.344935
1547.953379	96.668142	65.349940
1547.114573	106.913856	65.354945
1546.714270	99.113578	65.359950
1545.640826	89.870194	65.364954
1544.717986	93.973156	65.369959
1544.520595	89.800558	65.374964
1543.697001	106.832278	65.379969
1543.614241	82.954251	65.384974
1542.264378	95.827800	65.389978
1541.265828	95.470792	65.394983
1540.957356	88.873274	65.399988
1540.552093	97.307659	65.404993
1540.378820	94.473144	65.409998
1539.603357	91.388975	65.415002
1538.779336	91.105157	65.420007
1538.282504	93.010085	65.425012
1536.861147	97.567553	65.430017
1536.215859	90.358112	65.435022
1535.578565	93.392319	65.440026
1534.964820	101.104512	65.445031
1535.053046	82.022968	65.450036
1533.857656	93.161072	65.455041
1533.305458	90.202272	65.460046
1532.230892	93.990319	65.465050
1531.810509	98.054450	65.470055
1531.542538	87.859967	65.475060
1530.182926	105.747944	65.480065
1529.623247	96.761958	65.485070
1529.031245	88.952727	65.490074
1528.559434	89.626876	65.495079
1528.649677	90.452981	65.500084
1527.307631	93.562901	65.505089
1526.706596	91.384528	65.510094
1526.117835	96.065162	65.515098
1525.607176	96.639834	65.520103
1524.618712	90.492544	65.525108
1523.439515	96.476453	65.530113
1523.091638	86.944339	65.535118
1522.841253	94.825864	65.540122
1521.995437	96.677441	65.545127
1521.103184	84.469153	65.550132
1520.334841	99.314433	65.555137
1520.403411	82.066761	65.560142
1519.538064	88.081219	65.565146
1518.543553	86.815302	65.570151
1517.854028	82.823403	65.575156
1517.246077	101.118617	65.580161
1516.945907	85.747662	65.585166
1516.481326	91.047196	65.590170
1515.242878	92.554331	65.595175
1514.722888	78.151820	65.600180
1514.277731	95.003556	65.605185
1513.378686	85.711980	65.610190
1512.222666	94.587339	65.615194
1511.872139	103.389903	65.620199
1511.393412	89.802374	65.625204
1510.644561	96.298194	65.630209
1510.469164	84.324492	65.635214
1509.652887	79.397156	65.640218
1508.775379	85.315783	65.645223
1507.975263	75.158565	65.650228
1507.771879	86.973207	65.655233
1506.983363	89.664039	65.660238
1506.064083	86.276323	65.665242
1505.536067	97.742034	65.670247
1504.939052	96.442920	65.675252
1504.035577	94.577524	65.680257
1503.199181	81.705970	65.685262
1502.706938	89.263244	65.690266
1501.843009	92.052788	65.695271
1501.760339	85.463551	65.700276
1500.935050	86.198603	65.705281
1500.602352	83.547114	65.710286
1499.945219	90.818371	65.715290
1499.037864	87.431917	65.720295
1497.864789	79.499004	65.725300
1497.036723	98.131950	65.730305
1497.116324	90.225470	65.735310
1496.184935	87.282782	65.740314
1495.813235	94.710524	65.745319
1495.002368	86.682208	65.750324
1494.132858	97.379059	65.755329
1493.563503	85.277160	65.760334
1492.901674	92.263752	65.765338
1492.622043	91.783062	65.770343
1491.860389	81.211326	65.775348
1490.950277	94.495959	65.780353
1490.444069	92.865469	65.785358
1489.260844	86.768067	65.790362
1488.162210	98.986739	65.795367
1488.162542	85.810349	65.800372
1487.572658	90.576317	65.805377
1487.646182	91.868676	65.810382
1486.851776	96.208277	65.815386
1485.862361	93.782565	65.820391
1485.203869	83.355277	65.825396
1484.237263	92.312503	65.830401
1483.224887	83.743811	65.835406
1482.560795	89.269007	65.840410
1482.496484	90.255281	65.845415
1482.116616	87.772130	65.850420
1481.313340	98.150970	65.855425
1480.819070	89.036345	65.860430
1479.724537	85.211314	65.865434
1479.295976	93.217341	65.870439
1478.477604	96.706090	65.875444
1477.161601	94.597193	65.880449
1476.831979	85.510021	65.885454
1476.445113	83.724960	65.890458
1476.138400	86.473269	65.895463
1475.456725	87.660145	65.900468
1473.956329	97.515865	65.905473
1473.835736	91.940273	65.910478
1473.365507	95.465158	65.915482
1472.606158	93.352956	65.920487
1471.854390	90.309197	65.925492
1470.907401	93.264906	65.930497
1470.466563	87.644019	65.935502
1470.260676	83.472782	65.940506
1468.929847	97.120730	65.945511
1468.173324	89.522156	65.950516
1467.610661	90.403132	65.955521
1467.369131	88.740047	65.960526
1466.725975	89.340517	65.965530
1465.580726	91.786868	65.970535
1465.106790	79.871660	65.975540
1464.466007	96.128468	65.980545
1464.067996	93.285523	65.985550
1463.276794	87.389173	65.990554
1462.183048	88.165323	65.995559
1461.748813	76.926592	66.000564
1461.134039	91.028417	66.005569
1461.080342	80.292151	66.010574
1460.216543	89.479035	66.015578
1459.173214	92.085802	66.020583
1459.049711	90.940096	66.025588
1457.665036	95.742496	66.030593
1456.879833	89.498284	66.035598
1456.386912	88.400248	66.040602
1455.918309	86.446839	66.045607
1455.799018	91.333559	66.050612
1455.001675	87.986406	66.055617
1453.945087	90.887002	66.060622
1453.603963	93.727511	66.065626
1452.783186	89.299197	66.070631
1452.343691	92.899621	66.075636
1450.801226	91.175215	66.080641
1450.481654	91.155016	66.085646
1450.435128	87.552933	66.090650
1449.185503	82.065317	66.095655
1448.536493	89.800466	66.100660
1447.733408	89.013484	66.105665
1447.681713	90.142824	66.110670
1447.355421	86.045915	66.115674
1445.686214	89.685657	66.120679
1445.248432	88.862697	66.125684
1444.898577	93.797097	66.130689
1444.060918	87.105512	66.135694
1443.096058	86.402585	66.140698
1442.500128	100.616537	66.145703
1442.145477	86.769631	66.150708
1441.297248	94.257340	66.155713
1441.086041	92.009151	66.160718
1440.131498	92.457275	66.165722
1439.293304	106.473205	66.170727
1439.189378	88.100261	66.175732
1438.434470	90.708504	66.180737
1437.535357	90.332580	66.185742
1436.582687	97.284986	66.190746
1435.881930	95.418935	66.195751
1435.749437	81.867872	66.200756
1434.639901	92.006823	66.205761
1433.837378	84.286272	66.210766
1433.327227	83.982567	66.215770
1432.540134	96.320465	66.220775
1432.769338	91.851436	66.225780
1431.454735	99.444807	66.230785
1430.606455	100.904165	66.235790
1430.205448	99.026744	66.240794
1429.585864	88.985930	66.245799
1429.530071	95.094092	66.250804
1428.070950	98.990602	66.255809
1427.508074	87.412792	66.260814
1427.205931	82.777491	66.265818
1426.236441	90.508388	66.270823
1425.304975	87.162063	66.275828
1424.684682	92.497394	66.280833
1424.224271	96.284062	66.285838
1423.941839	89.710811	66.290842
1422.823848	98.536007	66.295847
1422.330755	86.094024	66.300852
1421.641021	85.624908	66.305857
1421.390541	88.958764	66.310862
1420.141338	83.847966	66.315866
1419.386191	90.076737	66.320871
1419.177689	85.642585	66.325876
1418.452275	97.075023	66.330881
1417.257519	88.289356	66.335886
1416.640558	86.148234	66.340890
1415.989495	99.084226	66.345895
1415.917317	89.085718	66.350900
1415.408004	99.397352	66.355905
1414.413362	96.977229	66.360910
1413.690811	86.739910	66.365914
1413.039323	84.832923	66.370919
1412.629252	91.183460	66.375924
1411.665511	100.280596	66.380929
1410.838847	85.918972	66.385934
1410.047681	92.833099	66.390938
1409.692207	101.451959	66.395943
1409.474187	88.510544	66.400948
1408.700689	96.580863	66.405953
1407.668169	84.634607	66.410958
1407.380493	90.401172	66.415962
1406.449236	100.574878	66.420967
1405.618988	88.590163	66.425972
1405.254400	96.149237	66.430977
1404.372817	104.271431	66.435982
1403.819827	89.647125	66.440986
1402.621403	94.052538	66.445991
1402.299213	87.001513	66.450996
1401.717481	92.989850	66.456001
1401.190093	90.449739	66.461006
1401.311911	91.688690	66.466010
1399.757678	96.868132	66.471015
1399.088286	87.454955	66.476020
1398.350222	88.439512	66.481025
1398.047761	84.384553	66.486030
1397.016498	92.363385	66.491034
1395.940293	94.021397	66.496039
1395.804420	85.034329	66.501044
1395.591895	89.229430	66.506049
1394.848726	96.118588	66.511054
1393.704172	89.723369	66.516058
1393.255588	93.110791	66.521063
1392.748920	91.477241	66.526068
1391.508409	81.650249	66.531073
1390.391129	95.371509	66.536078
1390.374638	89.088713	66.541082
1389.600726	84.921043	66.546087
1389.624476	71.622692	66.551092
1388.990695	87.091527	66.556097
1388.392910	92.677163	66.561102
1387.640639	91.088959	66.566106
1386.790774	97.214530	66.571111
1386.018704	89.667341	66.576116
1385.185262	90.771136	66.581121
1384.563827	77.639982	66.586126
1383.980858	92.435310	66.591130
1383.140679	93.842934	66.596135
1382.463661	93.625682	66.601140
1381.574195	88.484532	66.606145
1381.218131	81.361632	66.611150
1380.978330	98.390451	66.616154
1380.263538	89.068070	66.621159
1379.368491	75.039022	66.626164
1378.751998	95.391822	66.631169
1378.466775	85.747289	66.636174
1377.304453	79.194067	66.641178
1376.152955	93.461632	66.646183
1375.922787	80.405475	66.651188
1375.440350	79.982265	66.656193
1374.738624	78.810209	66.661198
1374.661297	85.949903	66.666202
1373.213139	96.432844	66.671207
1373.103853	81.922523	66.676212
1371.835393	91.146943	66.681217
1370.932387	89.261024	66.686222
1370.871008	86.503354	66.691226
1369.965643	95.641679	66.696231
1369.988107	89.869905	66.701236
1368.944171	86.358563	66.706241
1367.589712	88.901284	66.711246
1367.496396	93.608842	66.716250
1366.863207	82.907933	66.721255
1366.572262	80.730773	66.726260
1365.338864	93.347768	66.731265
1364.619014	84.371533	66.736270
1364.394403	84.008262	66.741274
1363.722142	82.922983	66.746279
1362.812523	108.499244	66.751284
1362.315683	86.561982	66.756289
1361.670207	82.731855	66.761294
1360.831964	88.850851	66.766298
1359.182588	96.880644	66.771303
1359.466574	90.453898	66.776308
1358.838364	95.207060	66.781313
1358.477922	93.566042	66.786318
1358.280888	91.738210	66.791322
1356.894093	93.209078	66.796327
1356.175721	86.399224	66.801332
1355.823839	87.300331	66.806337
1355.042201	88.932034	66.811342
1354.278661	88.570857	66.816346
1353.317382	103.227648	66.821351
1353.190870	80.742703	66.826356
1351.938982	84.972140	66.831361
1350.995127	85.033843	66.836366
1350.630705	77.054466	66.841370
1350.235871	79.195508	66.846375
1349.999999	84.149639	66.851380
1349.118041	85.308462	66.856385
1348.243571	70.170781	66.861390
1347.724624	94.210549	66.866394
1347.306150	94.362194	66.871399
1346.712503	79.689192	66.876404
1345.272577	78.759062	66.881409
1344.902798	89.458498	66.886414
1344.594531	83.838644	66.891418
1343.511836	98.424851	66.896423
1342.854334	83.810880	66.901428
1342.014522	78.840041	66.906433
1341.624591	82.267027	66.911438
1341.474766	82.724454	66.916442
1340.642099	82.438921	66.921447
1339.707487	95.270189	66.926452
1339.335370	89.077044	66.931457
1338.551003	83.824593	66.936462
1337.990582	70.324240	66.941466
1336.956849	92.637176	66.946471
1336.389735	74.408865	66.951476
1335.805718	78.074849	66.956481
1334.722350	77.045469	66.961486
1334.052919	75.609686	66.966490
1333.452729	75.899023	66.971495
1332.974150	75.432632	66.976500
1332.554610	80.985207	66.981505
1332.030274	81.659856	66.986510
1331.279060	73.973771	66.991514
1330.166637	80.445422	66.996519
1330.059241	68.088820	67.001524
1329.402934	75.318969	67.006529
1328.155850	75.695374	67.011534
1327.968651	76.388965	67.016538
1327.186417	83.500372	67.021543
1326.787681	75.535917	67.026548
1325.823984	81.744245	67.031553
1325.115677	84.107002	67.036558
1324.755595	77.095135	67.041562
1323.856946	85.190091	67.046567
1323.239157	79.975818	67.051572
1322.240427	73.593729	67.056577
1321.809205	79.539224	67.061582
1321.605692	82.028303	67.066586
1320.468802	85.397428	67.071591
1319.643567	79.621656	67.076596
1319.270307	78.960340	67.081601
1318.592505	74.824724	67.086606
1318.156459	79.418038	67.091610
1316.975415	84.024137	67.096615
1316.413069	74.814742	67.101620
1316.150949	79.952807	67.106625
1315.508695	83.345796	67.111630
1314.737095	78.791454	67.116634
1313.712868	85.100867	67.121639
1313.407881	71.518917	67.126644
1313.035584	78.721265	67.131649
1312.000494	86.013216	67.136654
1311.302236	76.355522	67.141658
1310.424187	82.502933	67.146663
1310.148610	73.337833	67.151668
1309.057098	76.895278	67.156673
1308.127550	91.051886	67.161678
1307.831999	61.952104	67.166682
1307.311944	79.216248	67.171687
1307.386583	86.730727	67.176692
1306.501680	69.210508	67.181697
1305.423200	85.915346	67.186702
1305.001102	75.635043	67.191706
1304.048984	73.206633	67.196711
1302.874133	85.346006	67.201716
1302.409769	81.476066	67.206721
1301.965323	82.138020	67.211726
1301.735608	82.844679	67.216730
1300.410066	80.376294	67.221735
1299.526133	84.386417	67.226740
1299.210238	81.801671	67.231745
1298.708706	85.303172	67.236750
1298.251162	79.798517	67.241754
1297.899992	89.140471	67.246759
1297.443744	81.675568	67.251764
1296.125520	78.097486	67.256769
1295.381194	86.301949	67.261774
1294.698100	85.404482	67.266778
1293.399163	89.829073	67.271783
1293.325983	87.030708	67.276788
1293.013543	84.191538	67.281793
1292.397853	80.965366	67.286798
1292.112158	75.409741	67.291802
1290.864162	82.634625	67.296807
1290.242108	83.487235	67.301812
1289.930062	89.357023	67.306817
1288.471509	80.361074	67.311822
1288.182526	84.759134	67.316826
1287.147572	85.308402	67.321831
1286.960814	87.276032	67.326836
1286.898121	72.933362	67.331841
1285.658905	80.558952	67.336846
1284.799001	75.572409	67.341850
1284.352732	84.040128	67.346855
1283.352595	79.597820	67.351860
1282.583265	86.130056	67.356865
1281.818691	90.419237	67.361870
1281.584368	77.087814	67.366874
1281.229210	85.717658	67.371879
1280.230796	84.897133	67.376884
1279.626194	77.350173	67.381889
1278.977102	83.305082	67.386894
1278.585908	92.011618	67.391898
1277.489241	86.405163	67.396903
1277.132568	78.755711	67.401908
1276.591518	84.004355	67.406913
1275.878406	84.112973	67.411918
1275.050407	79.211241	67.416922
1274.128262	94.888356	67.421927
1273.311490	87.245823	67.426932
1272.872681	83.226755	67.431937
1272.298173	90.240500	67.436942
1271.730076	86.923192	67.441946
1270.870411	90.380718	67.446951
1270.713792	86.994835	67.451956
1270.237414	77.327110	67.456961
1269.068151	94.443769	67.461966
1268.825432	87.671855	67.466970
1267.679905	93.010303	67.471975
1266.113368	84.398944	67.476980
1266.034760	84.271074	67.481985
1265.471039	86.755930	67.486990
1265.352589	85.032301	67.491994
1264.348483	91.150887	67.496999
1264.276524	82.189947	67.502004
1263.046022	88.691438	67.507009
1262.511098	85.980681	67.512014
1262.121843	84.383683	67.517018
1260.989554	82.759751	67.522023
1260.376077	90.648546	67.527028
1259.553060	87.015400	67.532033
1258.882681	85.089383	67.537038
1258.930300	91.368740	67.542042
1257.600513	89.139157	67.547047
1256.933805	84.143980	67.552052
1256.623757	84.620579	67.557057
1255.957316	91.000853	67.562062
1255.423829	85.533512	67.567066
1254.479654	87.077552	67.572071
1253.976631	89.366690	67.577076
1253.483389	87.989641	67.582081
1252.356947	81.951144	67.587086
1251.523416	82.548821	67.592090
1250.820723	96.186857	67.597095
1250.672940	79.448268	67.602100
1250.442410	90.811503	67.607105
1249.350571	79.469245	67.612110
1248.844280	94.170394	67.617114
1248.061691	89.483786	67.622119
1246.921719	90.382486	67.627124
1246.273249	100.582227	67.632129
1245.633872	87.096024	67.637134
1245.274541	83.600457	67.642138
1244.758547	96.918667	67.647143
1244.330133	91.537115	67.652148
1243.247014	85.021827	67.657153
1242.548290	83.417271	67.662158
1242.491671	80.349787	67.667162
1241.234001	92.376205	67.672167
1240.085495	88.324914	67.677172
1239.945774	83.550285	67.682177
1239.002469	88.892856	67.687182
1238.874353	78.928504	67.692186
1238.300738	90.995957	67.697191
1237.304191	90.913124	67.702196
1237.023486	77.354134	67.707201
1236.149802	88.750249	67.712206
1234.891566	82.518262	67.717210
1234.347073	83.319131	67.722215
1234.182241	88.723992	67.727220
1233.721332	93.600378	67.732225
1232.976052	84.552547	67.737230
1232.065070	84.974899	67.742234
1231.512226	97.827487	67.747239
1230.956615	96.909766	67.752244
1229.913375	84.027076	67.757249
1228.881448	96.757156	67.762254
1228.267994	83.143845	67.767258
1228.117153	100.193198	67.772263
1227.791352	88.707063	67.777268
1227.350949	94.756529	67.782273
1226.371932	101.065097	67.787278
1225.571511	98.812854	67.792282
1224.442459	95.215766	67.797287
1223.518981	94.835908	67.802292
1223.114730	106.217315	67.807297
1222.307201	104.850824	67.812302
1222.298129	86.745112	67.817306
1222.007322	99.068785	67.822311
1221.075970	93.918589	67.827316
1220.420722	85.457232	67.832321
1219.315618	96.432864	67.837326
1219.618388	89.610488	67.842330
1218.109401	94.978365	67.847335
1217.117362	82.092273	67.852340
1216.716786	93.507777	67.857345
1216.339740	99.006308	67.862350
1215.392952	96.242787	67.867354
1214.519846	91.483856	67.872359
1213.996888	86.412220	67.877364
1213.897971	87.369309	67.882369
1213.255736	98.884743	67.887374
1212.562421	92.411556	67.892378
1211.645976	99.457611	67.897383
1211.073400	87.203367	67.902388
1210.199316	80.870888	67.907393
1208.817661	97.242370	67.912398
1208.752196	91.497201	67.917402
1208.026414	87.796576	67.922407
1207.714291	90.345508	67.927412
1207.585371	91.554936	67.932417
1206.235599	87.529359	67.937422
1205.730707	88.579388	67.942426
1205.041953	82.066061	67.947431
1204.395806	93.995252	67.952436
1203.575387	88.171450	67.957441
1202.563962	94.909352	67.962446
1202.544251	78.681813	67.967450
1202.130050	87.888721	67.972455
1201.103840	86.695777	67.977460
1200.382617	89.155231	67.982465
1199.389937	97.873848	67.987470
1199.418460	90.317687	67.992474
1198.210214	93.081657	67.997479
1197.320954	88.191269	68.002484
1196.819126	85.268696	68.007489
1196.529416	90.434811	68.012494
1196.134412	82.969656	68.017498
1195.016024	88.973980	68.022503
1194.462253	84.254161	68.027508
1194.016973	74.319755	68.032513
1192.877972	92.384044	68.037518
1192.196076	79.912245	68.042522
1191.506761	78.068102	68.047527
1190.892345	87.224852	68.052532
1191.143535	81.667439	68.057537
1189.734393	98.481668	68.062542
1188.835571	87.105590	68.067546
1188.314381	86.936146	68.072551
1187.833075	95.079886	68.077556
1187.686811	94.108118	68.082561
1186.381483	89.302821	68.087566
1186.098046	91.191219	68.092570
1185.358272	93.391869	68.097575
1184.727704	93.621420	68.102580
1183.645598	96.191882	68.107585
1183.140467	92.774701	68.112590
1182.828313	88.644051	68.117594
1181.859182	89.119820	68.122599
1181.098026	93.408483	68.127604
1180.752897	90.943514	68.132609
1179.946149	88.772715	68.137614
1179.163651	76.491954	68.142618
1178.214413	101.979905	68.147623
1177.632586	85.997864	68.152628
1177.509311	83.648994	68.157633
1176.747934	87.070418	68.162638
1175.843454	92.447834	68.167642
1175.007595	86.128210	68.172647
1174.691366	90.055976	68.177652
1174.176024	80.487508	68.182657
1173.191517	95.684156	68.187662
1172.272167	90.189894	68.192666
1172.224078	82.912412	68.197671
1171.420999	85.164131	68.202676
1170.538569	80.715769	68.207681
1169.546209	91.131042	68.212686
1169.254099	80.825371	68.217690
1168.927076	94.936652	68.222695
1168.382896	85.133086	68.227700
1167.651699	89.342875	68.232705
1166.494096	91.337180	68.237710
1165.995118	87.980523	68.242714
1165.379051	94.855824	68.247719
1164.314626	96.873157	68.252724
1163.862800	89.577883	68.257729
1163.334172	89.676116	68.262734
1163.231920	83.358097	68.267738
1162.161736	92.886939	68.272743
1161.183283	89.133476	68.277748
1160.608327	85.762098	68.282753
1160.010594	96.470989	68.287758
1159.639180	85.000013	68.292762
1158.722192	89.685603	68.297767
1157.927146	86.696136	68.302772
1157.789887	74.606068	68.307777
1156.688531	81.899144	68.312782
1155.916235	83.463190	68.317786
1155.002994	85.606284	68.322791
1154.050623	90.702756	68.327796
1154.003666	81.722086	68.332801
1153.692517	82.979418	68.337806
1153.404726	84.136847	68.342810
1152.560030	82.744755	68.347815
1151.899841	97.746337	68.352820
1150.742818	92.252038	68.357825
1149.739512	97.180006	68.362830
1149.368496	93.197485	68.367834
1148.822220	94.736627	68.372839
1148.417844	88.059825	68.377844
1147.498422	87.259904	68.382849
1146.464730	91.830026	68.387854
1146.264828	89.236316	68.392858
1146.101686	95.951284	68.397863
1144.950413	79.343932	68.402868
1144.269551	86.100234	68.407873
1143.425709	92.166565	68.412878
1142.996774	76.913972	68.417882
1142.098694	84.072230	68.422887
1141.322530	94.098335	68.427892
1141.064441	92.389038	68.432897
1140.205612	95.811781	68.437902
1139.963315	83.178628	68.442906
1138.797337	80.262354	68.447911
1138.043308	86.494163	68.452916
1138.013952	88.614952	68.457921
1136.967548	90.268328	68.462926
1136.239020	85.114297	68.467930
1135.483975	91.667949	68.472935
1134.987129	78.442964	68.477940
1134.527416	85.720728	68.482945
1133.262586	84.083244	68.487950
1132.645406	92.245445	68.492954
1132.319983	91.060915	68.497959
1131.950041	89.855082	68.502964
1131.499565	93.058348	68.507969
1130.263400	96.312462	68.512974
1130.031607	87.600871	68.517978
1129.412326	82.256013	68.522983
1127.881317	92.154608	68.527988
1127.500840	89.597504	68.532993
1126.924050	89.837438	68.537998
1126.827166	76.665532	68.543002
1125.553653	80.862240	68.548007
1124.804159	86.522507	68.553012
1124.269353	81.353439	68.558017
1123.681641	94.448107	68.563022
1123.459231	89.487956	68.568026
1122.616575	85.903712	68.573031
1121.724328	83.186747	68.578036
1121.432692	74.796901	68.583041
1120.085474	86.755604	68.588046
1119.186944	85.537656	68.593050
1119.017404	81.567252	68.598055
1117.917595	86.985211	68.603060
1118.243571	81.188834	68.608065
1117.484743	89.289991	68.613070
1116.799137	77.443252	68.618074
1115.858388	86.375964	68.623079
1115.239196	92.753482	68.628084
1114.514760	85.288705	68.633089
1113.522655	86.643311	68.638094
1112.835719	95.409511	68.643098
1112.414494	89.047616	68.648103
1111.981944	83.753483	68.653108
1111.620766	75.541847	68.658113
1110.540619	78.492047	68.663118
1109.899905	76.665428	68.668122
1109.008177	102.377614	68.673127
1108.208480	79.640292	68.678132
1107.574094	83.096725	68.683137
1106.398525	88.941453	68.688142
1106.252451	81.624373	68.693146
1106.273223	87.026520	68.698151
1105.903756	83.351252	68.703156
1105.002117	82.032885	68.708161
1104.242832	85.367268	68.713166
1103.809199	77.421032	68.718170
1102.530260	86.448537	68.723175
1101.549883	82.542452	68.728180
1101.311520	80.765372	68.733185
1100.962505	95.635466	68.738190
1100.059711	93.021103	68.743194
1099.127609	94.596393	68.748199
1098.505394	89.576842	68.753204
1098.050631	83.349590	68.758209
1097.200948	86.316753	68.763214
1096.271367	83.482740	68.768218
1095.564856	76.860321	68.773223
1095.236262	84.946661	68.778228
1095.285927	86.793122	68.783233
1094.452652	82.874680	68.788238
1093.527670	87.334493	68.793242
1092.874874	90.937353	68.798247
1092.030530	97.005357	68.803252
1091.402095	80.417371	68.808257
1090.338412	97.031615	68.813262
1090.470537	85.327608	68.818266
1089.939603	86.873781	68.823271
1088.535371	97.189024	68.828276
1088.294723	87.151132	68.833281
1087.381647	89.104999	68.838286
1086.373919	97.718816	68.843290
1085.855560	95.085885	68.848295
1085.136046	89.682869	68.853300
1084.948064	80.923323	68.858305
1084.317345	90.123680	68.863310
1083.365611	77.051491	68.868314
1082.725302	90.274366	68.873319
1081.755570	99.538115	68.878324
1081.586358	88.954305	68.883329
1081.285805	87.399994	68.888334
1080.174554	79.052223	68.893338
1079.496082	81.433948	68.898343
1078.912336	83.855797	68.903348
1078.047267	78.138492	68.908353
1076.928155	95.974159	68.913358
1076.230690	79.510695	68.918362
1075.857287	78.828940	68.923367
1075.582673	85.637323	68.928372
1075.270949	81.847226	68.933377
1074.301172	89.401663	68.938382
1073.768580	80.559749	68.943386
1073.103205	82.945700	68.948391
1072.548675	83.218373	68.953396
1071.494309	77.271001	68.958401
1070.315990	87.750570	68.963406
1070.093047	79.398689	68.968410
1070.307457	80.976106	68.973415
1069.121921	90.029767	68.978420
1068.042425	78.887485	68.983425
1067.281883	73.916759	68.988430
1067.064690	98.935052	68.993434
1066.585845	82.331164	68.998439
1065.442292	93.407569	69.003444
1064.798491	89.772792	69.008449
1064.137165	89.802273	69.013454
1063.790355	84.764155	69.018458
1063.084400	84.360792	69.023463
1061.949680	87.048474	69.028468
1062.062893	83.544000	69.033473
1061.122485	85.101701	69.038478
1060.155754	78.911748	69.043482
1059.523578	92.347787	69.048487
1059.072272	83.554443	69.053492
1058.747767	78.151679	69.058497
1057.392678	88.113779	69.063502
1056.522705	72.710617	69.068506
1056.297067	90.751063	69.073511
1055.623951	92.001335	69.078516
1055.697695	82.709756	69.083521
1054.336102	88.962543	69.088526
1053.715942	79.901190	69.093530
1053.213039	80.023738	69.098535
1052.403131	81.921783	69.103540
1051.702281	75.109256	69.108545
1050.599977	79.556290	69.113550
1050.150803	83.044769	69.118554
1050.060047	79.856578	69.123559
1049.419160	81.814464	69.128564
1048.735247	74.729601	69.133569
1047.817397	80.602734	69.138574
1047.307593	77.602623	69.143578
1046.417058	87.885042	69.148583
1045.532226	80.873138	69.153588
1045.280452	79.768363	69.158593
1045.096873	79.888997	69.163598
1043.877748	80.157019	69.168602
1043.209300	80.613390	69.173607
1042.237842	87.346559	69.178612
1042.046015	88.215937	69.183617
1040.798805	85.300018	69.188622
1040.075316	86.280780	69.193626
1039.710211	81.217194	69.198631
1038.966065	94.327293	69.203636
1038.993462	72.352528	69.208641
1037.918553	83.697119	69.213646
1037.035469	80.306987	69.218650
1036.849594	92.582420	69.223655
1036.193149	77.998376	69.228660
1035.207881	74.799532	69.233665
1034.152321	88.421187	69.238670
1033.770374	92.198580	69.243674
1033.611896	78.434128	69.248679
1032.891281	85.015437	69.253684
1032.039863	78.233176	69.258689
1031.199381	82.107165	69.263694
1030.850597	80.188396	69.268698
1029.907379	80.142890	69.273703
1028.752059	93.427204	69.278708
1028.557505	94.126716	69.283713
1028.144595	92.263877	69.288718
1027.409759	97.548122	69.293722
1026.313311	80.427528	69.298727
1025.797245	85.801538	69.303732
1025.629800	80.690742	69.308737
1025.005477	89.888514	69.313742
1024.136130	91.791294	69.318746
1023.914748	83.664661	69.323751
1022.672729	91.073201	69.328756
1022.053295	81.131855	69.333761
1020.811938	94.366786	69.338766
1020.254049	79.637766	69.343770
1019.930973	85.198681	69.348775
1019.552745	97.627713	69.353780
1019.255107	86.914545	69.358785
1018.117614	89.405579	69.363790
1017.420893	76.606649	69.368794
1017.052899	79.724271	69.373799
1015.692829	73.735680	69.378804
1014.691704	84.273804	69.383809
1014.367413	83.037074	69.388814
1014.007884	79.525814	69.393818
1013.924469	73.911250	69.398823
1012.982007	83.411930	69.403828
1012.276564	85.105722	69.408833
1011.840179	86.723595	69.413838
1010.733041	92.794005	69.418842
1009.717814	78.986099	69.423847
1009.122463	73.465596	69.428852
1008.672471	90.149364	69.433857
1008.135086	66.077364	69.438862
1007.987668	96.832185	69.443866
1007.088590	75.294961	69.448871
1006.206646	82.231504	69.453876
1005.780281	84.776554	69.458881
1004.921268	73.061524	69.463886
1003.590151	82.141520	69.468890
1003.341402	87.703227	69.473895
1002.942237	88.630823	69.478900
1002.439856	77.112928	69.483905
1001.658760	93.325860	69.488910
1000.924396	96.254207	69.493914
1000.622403	74.268778	69.498919
999.545665	82.655486	69.503924
998.771771	71.283289	69.508929
997.836236	92.090524	69.513934
997.514275	79.343934	69.518938
997.282801	74.207063	69.523943
996.206064	97.473015	69.528948
995.693072	81.044889	69.533953
994.813663	76.211364	69.538958
994.715332	104.965240	69.543962
993.712880	65.797846	69.548967
992.677668	96.687602	69.553972
992.657353	75.879425	69.558977
991.885091	75.081380	69.563982
991.210823	97.110118	69.568986
990.659715	74.148829	69.573991
989.951934	73.991767	69.578996
988.763605	96.367203	69.584001
987.722432	76.361651	69.589006
987.233250	75.849709	69.594010
986.778283	71.114229	69.599015
986.550751	82.295632	69.604020
986.192442	79.522152	69.609025
985.104123	77.798318	69.614030
984.270964	82.144213	69.619034
984.087622	77.081682	69.624039
982.868115	88.029854	69.629044
982.199109	73.706440	69.634049
981.659696	89.970799	69.639054
981.152600	87.571054	69.644058
981.005650	71.898364	69.649063
979.664340	76.987387	69.654068
979.041178	85.360281	69.659073
978.590537	86.478987	69.664078
977.489100	76.899760	69.669082
976.624856	98.733236	69.674087
975.904539	84.909958	69.679092
975.719662	69.825167	69.684097
974.983192	81.719863	69.689102
974.656194	90.911335	69.694106
974.458079	80.428338	69.699111
973.780819	78.673798	69.704116
972.844372	73.914009	69.709121
971.362434	86.301034	69.714126
970.623207	88.805987	69.719130
970.400466	72.363236	69.724135
969.781819	73.958078	69.729140
969.458154	81.209479	69.734145
968.597511	82.823903	69.739150
967.660891	88.890849	69.744154
967.561842	74.238650	69.749159
966.727462	75.032084	69.754164
965.615198	81.384002	69.759169
964.690011	84.378986	69.764174
964.260514	81.973206	69.769178
964.071618	73.002533	69.774183
963.449336	90.041699	69.779188
962.696562	85.933889	69.784193
961.876640	80.322981	69.789198
961.393292	83.477886	69.794202
961.013428	81.313353	69.799207
959.498305	86.059483	69.804212
959.218387	78.377391	69.809217
958.657945	83.979231	69.814222
958.244984	78.805013	69.819226
957.663611	82.123740	69.824231
956.574563	81.232616	69.829236
956.270364	68.309766	69.834241
955.335420	73.819813	69.839246
954.145260	82.727600	69.844250
953.739486	77.813999	69.849255
953.002997	81.261480	69.854260
952.989290	76.421105	69.859265
952.535899	73.181820	69.864270
951.634427	83.653645	69.869274
951.109151	76.824254	69.874279
950.074091	80.142635	69.879284
949.231821	76.979419	69.884289
948.547575	87.855049	69.889294
947.881141	82.257568	69.894298
947.694750	78.182639	69.899303
946.251059	84.341311	69.904308
945.566216	78.835065	69.909313
945.157268	78.149525	69.914318
944.775740	79.813869	69.919322
944.623768	75.520589	69.924327
943.401082	77.597880	69.929332
942.810588	75.050576	69.934337
942.317533	75.088005	69.939342
941.670002	72.423629	69.944346
940.849066	75.958662	69.949351
939.862312	84.711095	69.954356
939.498001	70.200456	69.959361
938.975544	88.223465	69.964366
937.577870	88.469489	69.969370
937.241981	67.993809	69.974375
936.493049	82.392965	69.979380
936.398842	80.223981	69.984385
936.119194	85.186670	69.989390
934.901333	84.396471	69.994394
934.084313	77.115221	69.999399
933.476359	88.101710	70.004404
933.013967	78.819764	70.009409
931.665701	78.471339	70.014414
931.085673	71.888774	70.019418
930.928861	65.680389	70.024423
930.069786	83.832645	70.029428
929.948324	74.751904	70.034433
929.150230	69.128078	70.039438
927.963469	101.664549	70.044442
927.832992	67.305061	70.049447
926.958736	94.271218	70.054452
926.420988	68.778561	70.059457
925.477418	75.305486	70.064462
925.023664	89.443228	70.069466
924.462299	76.258545	70.074471
923.440782	77.289915	70.079476
922.659008	78.518088	70.084481
921.992543	93.558531	70.089486
921.909368	89.522367	70.094490
921.549163	84.935813	70.099495
919.878030	75.168169	70.104500
919.672455	84.766067	70.109505
919.052015	83.246914	70.114510
918.651536	68.614313	70.119514
917.556862	74.867259	70.124519
916.494887	88.450544	70.129524
916.464990	74.772887	70.134529
915.975123	80.631568	70.139534
914.904125	85.035829	70.144538
914.027520	87.253593	70.149543
913.402612	79.563334	70.154548
913.591920	76.772106	70.159553
912.873972	69.760515	70.164558
912.203828	90.445107	70.169562
911.530061	78.924552	70.174567
910.400250	77.934286	70.179572
909.187338	91.625168	70.184577
908.801944	69.014425	70.189582
907.900267	82.704654	70.194586
908.205482	73.622247	70.199591
906.843965	92.489945	70.204596
906.350786	73.753343	70.209601
906.061867	97.182506	70.214606
905.387249	64.131693	70.219610
904.579865	89.488269	70.224615
903.522352	58.146218	70.229620
903.213427	82.851063	70.234625
903.014081	73.159863	70.239630
901.667598	90.954483	70.244634
901.261444	84.383673	70.249639
900.600308	85.942718	70.254644
899.850995	75.265197	70.259649
899.045589	76.662707	70.264654
897.864192	89.104437	70.269658
897.743044	85.772867	70.274663
897.188109	83.412291	70.279668
896.750134	78.109612	70.284673
895.960074	74.821419	70.289678
894.824812	81.050875	70.294682
894.608565	75.358119	70.299687
894.244330	78.224436	70.304692
893.526880	74.938880	70.309697
892.476751	86.921354	70.314702
891.945720	83.598246	70.319706
891.370051	63.252205	70.324711
890.285603	91.418680	70.329716
889.482365	84.672960	70.334721
889.253032	74.721621	70.339726
888.584303	77.988035	70.344730
888.626947	66.875428	70.349735
887.075616	91.241871	70.354740
886.669407	73.079605	70.359745
885.866990	71.302434	70.364750
885.203878	93.889178	70.369754
884.283365	83.213672	70.374759
883.518934	83.839892	70.379764
883.114969	75.269288	70.384769
883.066129	69.917302	70.389774
882.562443	81.446982	70.394778
881.604891	75.014391	70.399783
881.110901	84.219822	70.404788
879.835078	79.313819	70.409793
878.926675	88.036458	70.414798
877.916219	83.947610	70.419802
877.821851	76.522993	70.424807
877.489122	81.768505	70.429812
877.233962	94.915919	70.434817
876.209448	75.691486	70.439822
874.992698	80.826965	70.444826
874.583785	84.118262	70.449831
874.385865	88.396208	70.454836
873.835109	82.938027	70.459841
872.662139	77.998314	70.464846
871.933560	89.276804	70.469850
872.105047	87.450291	70.474855
870.609396	91.374983	70.479860
869.996807	87.566573	70.484865
869.306632	71.571957	70.489870
869.036143	86.341233	70.494874
868.367877	85.968195	70.499879
867.330098	96.830727	70.504884
866.903541	84.258500	70.509889
866.296766	79.700161	70.514894
865.003601	81.509602	70.519898
864.846869	76.535886	70.524903
864.035418	84.317482	70.529908
863.459450	80.053844	70.534913
863.243433	75.326092	70.539918
861.848747	88.904000	70.544922
861.836998	80.496468	70.549927
860.648951	70.139512	70.554932
860.216407	82.734863	70.559937
859.497962	68.873509	70.564942
858.312387	78.278886	70.569946
858.035009	89.308960	70.574951
857.750096	77.162026	70.579956
857.324360	83.163464	70.584961
856.181594	87.039885	70.589966
855.218494	88.061986	70.594970
855.109922	75.620500	70.599975
854.684454	81.227681	70.604980
853.760833	73.105622	70.609985
852.871345	76.288913	70.614990
852.075113	82.740377	70.619994
851.888329	71.430911	70.624999
850.843343	76.723554	70.630004
850.132729	70.842999	70.635009
849.806209	90.873700	70.640014
849.139000	82.245656	70.645018
848.180310	71.719746	70.650023
847.349373	72.728699	70.655028
846.841343	78.683313	70.660033
846.687324	81.986081	70.665038
846.068782	78.713182	70.670042
845.166671	66.506807	70.675047
844.599196	74.823547	70.680052
843.663494	87.582557	70.685057
842.759608	76.852394	70.690062
841.981308	72.285097	70.695066
841.239517	90.238945	70.700071
841.305266	90.428713	70.705076
840.803556	69.544245	70.710081
840.191601	81.042277	70.715086
839.063065	89.520860	70.720090
838.783708	78.901019	70.725095
837.572184	69.829796	70.730100
836.329386	69.865157	70.735105
836.333196	84.833608	70.740110
835.674925	93.648906	70.745114
835.364256	69.947728	70.750119
834.549967	74.265429	70.755124
833.573166	83.924577	70.760129
833.192763	75.708182	70.765134
832.523815	84.665515	70.770138
831.755588	79.748130	70.775143
830.770088	68.029666	70.780148
829.930075	75.539862	70.785153
830.020531	76.580354	70.790158
829.078706	77.767801	70.795162
829.193408	81.601774	70.800167
827.946897	84.906552	70.805172
827.261127	78.624680	70.810177
826.808633	82.077451	70.815182
825.842819	80.115007	70.820186
825.047327	74.566494	70.825191
824.234252	91.960870	70.830196
823.933408	84.297901	70.835201
823.550612	77.278722	70.840206
822.650461	79.624835	70.845210
822.223116	78.346192	70.850215
820.999449	75.548062	70.855220
820.002994	92.899092	70.860225
819.722981	73.452125	70.865230
819.167423	86.108058	70.870234
818.892631	72.340097	70.875239
818.525317	78.940903	70.880244
817.635534	87.862431	70.885249
816.749269	76.639074	70.890254
815.811504	79.224550	70.895258
814.951528	73.889719	70.900263
814.270720	75.011973	70.905268
813.840456	91.784058	70.910273
813.570126	74.978361	70.915278
812.805489	80.842945	70.920282
811.915818	83.474381	70.925287
811.426795	75.652149	70.930292
810.772044	71.905661	70.935297
810.188001	77.132834	70.940302
808.658534	87.010839	70.945306
808.419618	83.144546	70.950311
807.863813	82.657435	70.955316
807.309903	78.067047	70.960321
807.119111	81.572776	70.965326
806.182833	72.125042	70.970330
805.446341	72.461427	70.975335
805.105232	87.582542	70.980340
804.124078	83.161077	70.985345
803.402324	74.770381	70.990350
802.795999	79.225290	70.995354
802.442760	80.621815	71.000359
801.316752	77.098565	71.005364
800.298592	78.151526	71.010369
800.066858	80.717660	71.015374
799.409919	81.604321	71.020378
799.062142	57.448643	71.025383
797.936357	83.272183	71.030388
796.944405	84.174326	71.035393
796.773046	79.253404	71.040398
796.170311	85.722966	71.045402
795.760586	80.105172	71.050407
794.818724	84.178282	71.055412
794.139589	84.153902	71.060417
793.636643	85.175315	71.065422
792.575873	80.482695	71.070426
791.814873	66.194512	71.075431
791.339549	74.777271	71.080436
790.866473	71.310934	71.085441
790.632228	85.115708	71.090446
789.675610	90.605609	71.095450
788.835621	82.408765	71.100455
788.292369	74.137885	71.105460
787.665071	78.362761	71.110465
786.841907	81.740508	71.115470
786.119641	94.025621	71.120474
785.544012	80.490040	71.125479
785.141699	87.154767	71.130484
783.995805	89.282984	71.135489
783.389489	82.740912	71.140494
782.414928	94.501672	71.145498
782.148038	77.521979	71.150503
781.825165	91.031803	71.155508
781.292792	84.843790	71.160513
780.300389	75.499612	71.165518
779.694405	84.533657	71.170522
779.359709	78.919693	71.175527
778.349105	89.765304	71.180532
777.582089	81.012835	71.185537
777.119117	77.128601	71.190542
776.310828	85.231393	71.195546
775.476301	79.998174	71.200551
774.931598	80.182620	71.205556
774.191572	93.539668	71.210561
774.143265	78.800584	71.215566
772.985885	93.532858	71.220570
772.216267	72.716292	71.225575
771.842062	86.243744	71.230580
771.465718	84.491819	71.235585
770.629465	83.155284	71.240590
769.537101	80.918136	71.245594
769.132933	79.351980	71.250599
768.378613	94.658720	71.255604
767.265993	97.210553	71.260609
766.354408	87.812510	71.265614
765.772717	92.235126	71.270618
766.046712	86.765523	71.275623
765.580726	85.037331	71.280628
764.911569	87.403459	71.285633
764.268268	76.529356	71.290638
763.397759	83.946662	71.295642
762.276066	85.492330	71.300647
761.136687	82.980413	71.305652
760.674723	78.889455	71.310657
760.610489	71.004348	71.315662
760.165056	81.378390	71.320666
759.503719	80.580105	71.325671
758.461763	84.826846	71.330676
757.984860	76.222157	71.335681
757.454212	78.676616	71.340686
756.075721	85.406864	71.345690
755.370083	81.386234	71.350695
755.227168	84.070688	71.355700
754.565309	72.986670	71.360705
753.980641	81.996824	71.365710
753.034898	89.921246	71.370714
752.283770	79.537367	71.375719
752.075787	82.044533	71.380724
751.499178	91.206366	71.385729
750.833438	74.919345	71.390734
749.762627	69.900362	71.395738
749.477302	83.423123	71.400743
748.709625	90.737340	71.405748
747.476497	87.232743	71.410753
747.024922	68.707195	71.415758
746.787208	96.519717	71.420762
746.303621	84.525851	71.425767
745.269831	81.492540	71.430772
744.080826	79.081566	71.435777
743.961660	80.368300	71.440782
743.590008	90.142438	71.445786
742.943884	79.997297	71.450791
741.873705	77.818128	71.455796
741.119573	80.722880	71.460801
741.038374	92.385580	71.465806
739.919102	86.839757	71.470810
739.149430	82.442996	71.475815
738.505050	82.031500	71.480820
737.959071	89.312001	71.485825
737.712071	80.604486	71.490830
736.501938	76.976396	71.495834
735.775084	86.740852	71.500839
735.388178	82.628488	71.505844
734.896630	86.461205	71.510849
734.265029	76.594437	71.515854
733.399889	81.107910	71.520858
732.911100	89.412146	71.525863
732.329147	82.104590	71.530868
731.231294	76.310953	71.535873
730.477676	87.167700	71.540878
729.987281	88.046787	71.545882
729.592111	89.073130	71.550887
728.837768	84.995611	71.555892
727.978631	87.871357	71.560897
727.764109	80.592034	71.565902
727.025437	81.176355	71.570906
726.055416	74.324800	71.575911
725.302449	90.410291	71.580916
724.669121	83.229181	71.585921
724.452033	77.377322	71.590926
723.139239	76.417850	71.595930
722.611589	81.941971	71.600935
721.882311	80.678302	71.605940
721.453666	81.853469	71.610945
721.447216	72.850638	71.615950
720.568217	86.143086	71.620954
719.540498	92.724475	71.625959
718.677417	88.088718	71.630964
718.228943	82.294195	71.635969
717.363002	83.239382	71.640974
716.484748	92.972759	71.645978
715.782950	85.917662	71.650983
715.949841	78.413625	71.655988
715.177140	88.689979	71.660993
714.260968	88.012696	71.665998
713.314678	67.561744	71.671002
713.120143	101.622767	71.676007
712.566538	63.836437	71.681012
711.561784	80.148074	71.686017
711.187772	76.352187	71.691022
710.264815	89.698944	71.696026
709.142585	80.383353	71.701031
708.541332	83.962321	71.706036
707.579629	78.287358	71.711041
707.305194	68.035756	71.716046
706.412433	98.615867	71.721050
706.675704	69.719083	71.726055
706.082046	66.741866	71.731060
705.471365	78.455737	71.736065
704.696142	71.661483	71.741070
703.847837	89.211281	71.746074
702.633539	67.672402	71.751079
701.913266	75.144644	71.756084
701.530209	83.860950	71.761089
701.521113	62.825586	71.766094
700.579047	89.179683	71.771098
699.389934	82.594817	71.776103
699.181477	71.134302	71.781108
698.630421	75.238253	71.786113
697.931578	82.360179	71.791118
697.044499	84.675870	71.796122
696.118969	73.682737	71.801127
696.173359	71.228353	71.806132
694.962723	82.504775	71.811137
694.372443	74.488977	71.816142
693.680303	91.231796	71.821146
693.486190	79.031024	71.826151
692.313767	71.934186	71.831156
691.403071	85.408293	71.836161
691.097436	80.522955	71.841166
690.605978	84.464467	71.846170
690.140209	75.399161	71.851175
689.061611	91.549119	71.856180
688.263178	91.682525	71.861185
688.180399	79.867701	71.866190
687.444230	83.157514	71.871194
686.462770	81.732171	71.876199
686.136159	74.093838	71.881204
685.247426	81.501451	71.886209
683.706612	81.089206	71.891214
683.225417	83.094286	71.896218
682.919495	83.608140	71.901223
682.636542	77.703700	71.906228
681.601365	82.447675	71.911233
681.682876	73.445034	71.916238
680.981422	74.781908	71.921242
680.157578	71.535438	71.926247
679.447711	72.058419	71.931252
678.519764	68.614075	71.936257
677.675267	64.599817	71.941262
677.173551	73.051178	71.946266
676.437091	80.574887	71.951271
676.447853	71.411636	71.956276
674.788823	70.116261	71.961281
674.620467	64.586217	71.966286
673.951220	91.215404	71.971290
673.452709	76.322535	71.976295
672.708769	71.767173	71.981300
671.695202	75.965272	71.986305
671.613895	73.042093	71.991310
671.011546	77.299287	71.996314
669.962796	74.366158	72.001319
669.221448	86.886117	72.006324
668.410121	79.589876	72.011329
668.061220	70.010839	72.016334
666.772685	82.480737	72.021338
666.356593	79.708629	72.026343
665.949834	76.367368	72.031348
665.253247	67.986913	72.036353
664.978676	80.284319	72.041358
664.398249	68.644936	72.046362
663.139096	78.599806	72.051367
662.886344	75.118914	72.056372
662.353699	62.655119	72.061377
661.551604	72.278605	72.066382
660.490251	82.384898	72.071386
659.869565	79.954432	72.076391
659.557848	64.654969	72.081396
658.772527	71.095277	72.086401
657.901051	90.875287	72.091406
657.439885	91.048034	72.096410
656.765431	66.472937	72.101415
656.526077	69.850793	72.106420
655.336044	89.925939	72.111425
654.946872	73.560233	72.116430
654.271067	78.193380	72.121434
653.289830	70.627757	72.126439
652.605042	88.884761	72.131444
651.880591	79.647778	72.136449
651.647936	76.591014	72.141454
651.043167	79.714842	72.146458
650.094950	82.606373	72.151463
649.633040	74.078171	72.156468
648.960451	77.578628	72.161473
648.308969	77.478926	72.166478
647.119644	87.955665	72.171482
646.610880	77.648349	72.176487
646.103396	72.807778	72.181492
645.542874	81.713184	72.186497
645.445129	83.982043	72.191502
644.415465	70.936690	72.196506
643.925030	72.350351	72.201511
643.188673	92.328031	72.206516
641.879479	80.946611	72.211521
641.389219	66.072949	72.216526
640.881905	81.974253	72.221530
640.490025	69.776609	72.226535
639.604043	66.070149	72.231540
638.816817	94.075795	72.236545
638.315273	72.879167	72.241550
637.891430	84.449765	72.246554
637.099188	63.327826	72.251559
636.191098	63.544938	72.256564
635.438841	85.472551	72.261569
635.065849	87.856200	72.266574
634.363704	80.739692	72.271578
633.540877	83.786292	72.276583
633.248893	63.354197	72.281588
632.568115	81.853389	72.286593
631.467224	85.598663	72.291598
630.782364	79.460207	72.296602
630.160068	77.211344	72.301607
630.063263	68.203991	72.306612
629.030528	93.296868	72.311617
628.221962	57.515969	72.316622
627.363589	81.174510	72.321626
626.929362	72.760171	72.326631
626.596793	63.270006	72.331636
625.445179	90.904770	72.336641
625.275564	65.175463	72.341646
624.401418	60.954649	72.346650
623.791262	77.361149	72.351655
623.533061	83.481002	72.356660
622.623006	85.582770	72.361665
621.984292	67.563282	72.366670
621.195611	69.558994	72.371674
619.890781	75.326731	72.376679
619.374150	70.930720	72.381684
618.975949	89.375462	72.386689
618.677282	77.885172	72.391694
617.981844	80.471548	72.396698
617.175470	83.409883	72.401703
616.474756	64.400551	72.406708
615.669683	81.415224	72.411713
615.513965	79.051064	72.416718
614.243158	75.286054	72.421722
613.440032	79.502698	72.426727
613.317130	69.356287	72.431732
612.597111	77.161222	72.436737
612.234952	74.326924	72.441742
611.209476	73.824773	72.446746
610.321421	63.685106	72.451751
610.170576	79.848165	72.456756
608.984572	79.633336	72.461761
608.235517	67.336475	72.466766
607.810796	75.446022	72.471770
607.345522	82.105020	72.476775
607.226378	77.372914	72.481780
605.869997	78.823567	72.486785
605.132934	90.314750	72.491790
604.642413	77.276588	72.496794
603.753372	77.329840	72.501799
603.155486	66.650410	72.506804
601.921477	94.869126	72.511809
602.109696	78.274295	72.516814
601.745936	68.041672	72.521818
600.912410	90.068964	72.526823
600.525458	61.952239	72.531828
599.365718	97.299107	72.536833
598.737395	69.873624	72.541838
597.709806	77.662895	72.546842
596.863432	76.031584	72.551847
596.772671	70.236895	72.556852
596.104583	66.084193	72.561857
595.516653	71.203218	72.566862
594.678266	75.988418	72.571866
594.096220	70.967360	72.576871
593.627101	67.492554	72.581876
592.335748	75.442095	72.586881
591.911654	78.977102	72.591886
591.305731	78.091195	72.596890
590.771959	72.704504	72.601895
590.462601	77.511102	72.606900
589.175711	73.811742	72.611905
589.006724	70.636045	72.616910
588.477333	75.890819	72.621914
587.084842	81.784492	72.626919
586.530900	74.923504	72.631924
585.695157	62.224175	72.636929
585.584619	81.474591	72.641934
585.058637	76.651173	72.646938
583.758963	64.039921	72.651943
583.262303	76.453111	72.656948
582.685321	74.933433	72.661953
582.827705	53.763607	72.666958
581.653955	77.272112	72.671962
580.513039	86.806093	72.676967
580.225927	69.038112	72.681972
579.322003	88.187826	72.686977
578.799868	54.146350	72.691982
577.707173	69.566899	72.696986
577.351384	74.486541	72.701991
577.361958	66.835531	72.706996
576.382300	73.762521	72.712001
575.330221	60.965197	72.717006
574.545809	87.732557	72.722010
573.909922	69.482418	72.727015
573.752498	87.040463	72.732020
573.017432	73.576092	72.737025
572.106125	63.296653	72.742030
571.574646	81.679037	72.747034
571.220078	87.237114	72.752039
570.695203	75.891667	72.757044
569.255534	72.170922	72.762049
569.021208	69.398269	72.767054
568.493891	82.724613	72.772058
567.674709	70.997142	72.777063
567.061903	72.073938	72.782068
566.075055	87.543879	72.787073
565.523584	82.003902	72.792078
565.344261	83.438986	72.797082
564.096916	75.669797	72.802087
563.584485	84.963345	72.807092
563.041299	80.447003	72.812097
562.076146	75.419165	72.817102
560.876107	73.689665	72.822106
560.370615	73.721265	72.827111
560.410457	66.106594	72.832116
559.861822	85.893535	72.837121
559.553521	75.644201	72.842126
558.670710	74.107011	72.847130
557.800501	101.566107	72.852135
557.492210	77.746382	72.857140
556.512343	74.114827	72.862145
555.889018	77.646880	72.867150
555.371859	81.822725	72.872154
554.319573	91.780966	72.877159
553.738594	69.384434	72.882164
552.984998	78.002077	72.887169
552.654548	69.282667	72.892174
551.566544	89.012026	72.897178
550.413364	64.505355	72.902183
550.236003	79.023245	72.907188
549.772743	91.558855	72.912193
549.425518	65.123052	72.917198
548.725218	69.454212	72.922202
547.641416	89.028371	72.927207
547.285293	76.082357	72.932212
546.455990	78.653804	72.937217
546.114923	67.555045	72.942222
545.041665	73.650184	72.947226
544.345658	76.443236	72.952231
544.111426	72.361785	72.957236
543.108425	75.579024	72.962241
542.112007	70.064200	72.967246
541.740104	73.653974	72.972250
540.770088	89.785096	72.977255
541.109938	68.903903	72.982260
539.934815	72.851833	72.987265
539.046434	73.788038	72.992270
538.544105	83.944092	72.997274
537.979472	78.797279	73.002279
537.174262	80.697885	73.007284
536.038091	82.381565	73.012289
535.840601	75.654615	73.017294
535.111134	84.842396	73.022298
534.965907	76.588615	73.027303
534.101170	66.402693	73.032308
533.210659	89.113957	73.037313
533.035953	73.758007	73.042318
532.107605	68.759014	73.047322
530.883277	79.586695	73.052327
530.484429	77.210810	73.057332
530.007228	77.692043	73.062337
529.426645	80.742663	73.067342
528.591640	77.330879	73.072346
527.734685	92.393816	73.077351
527.482258	86.344198	73.082356
527.016557	69.416757	73.087361
525.660959	95.560801	73.092366
525.137984	76.679295	73.097370
524.391508	83.378364	73.102375
524.173645	77.966600	73.107380
523.564197	87.816466	73.112385
522.577845	75.899610	73.117390
522.109698	86.121181	73.122394
521.288703	80.039137	73.127399
521.136465	73.803267	73.132404
519.884751	94.232031	73.137409
519.147759	79.210056	73.142414
518.711662	77.865060	73.147418
518.150932	86.650677	73.152423
517.496095	76.574814	73.157428
516.639806	73.480219	73.162433
516.069310	73.660946	73.167438
515.780298	78.708720	73.172442
514.382037	78.464673	73.177447
514.007238	64.373707	73.182452
513.551004	75.079042	73.187457
513.000457	80.792909	73.192462
512.479509	73.705930	73.197466
511.666421	74.218593	73.202471
510.820662	67.550763	73.207476
509.942311	65.907233	73.212481
508.797911	76.711150	73.217486
508.418976	73.841698	73.222490
507.550409	77.114802	73.227495
507.818900	77.964503	73.232500
507.209922	81.051187	73.237505
506.486114	75.737365	73.242510
505.591440	68.058683	73.247514
505.234785	81.971239	73.252519
504.447086	73.658967	73.257524
503.006269	82.619466	73.262529
502.271650	76.468483	73.267534
502.328614	66.302901	73.272538
501.548367	77.532906	73.277543
501.411421	74.041474	73.282548
500.113606	83.264605	73.287553
499.937008	72.078158	73.292558
499.526940	73.286667	73.297562
498.222493	72.870000	73.302567
497.473482	81.171556	73.307572
496.844296	86.606238	73.312577
496.263460	81.632317	73.317582
495.496954	67.166965	73.322586
494.290428	84.799081	73.327591
494.207816	77.858308	73.332596
493.593927	82.317636	73.337601
493.084239	85.394815	73.342606
492.674709	74.731143	73.347610
491.316207	78.687807	73.352615
491.257082	71.897827	73.357620
490.597403	76.752353	73.362625
489.448555	74.830243	73.367630
488.949568	71.576246	73.372634
488.294334	82.035763	73.377639
488.288503	78.288494	73.382644
486.667614	90.500771	73.387649
486.124719	81.091437	73.392654
485.508029	89.851284	73.397658
484.857326	86.077440	73.402663
484.560158	71.548361	73.407668
483.209812	68.201345	73.412673
482.517921	96.048316	73.417678
482.279616	69.964165	73.422682
481.937706	78.877338	73.427687
481.547286	89.829228	73.432692
480.423508	83.306610	73.437697
479.523817	72.407234	73.442702
479.113637	68.953025	73.447706
478.858729	91.446358	73.452711
477.871043	63.572034	73.457716
476.994015	81.197389	73.462721
476.619943	87.114948	73.467726
476.032341	83.901875	73.472730
474.742282	87.905990	73.477735
474.238768	76.809468	73.482740
473.815425	81.003495	73.487745
473.399487	71.515604	73.492750
472.587302	75.948181	73.497754
471.528597	79.365119	73.502759
471.047546	74.909864	73.507764
470.529154	80.216519	73.512769
470.001621	72.272796	73.517774
469.229466	77.686104	73.522778
468.287958	79.748783	73.527783
467.983360	75.303262	73.532788
467.638290	81.667178	73.537793
466.646097	80.462818	73.542798
466.205932	79.380236	73.547802
465.299466	82.588433	73.552807
464.403510	74.809053	73.557812
463.629346	82.083365	73.562817
463.262417	82.160715	73.567822
462.932904	64.971926	73.572826
461.690302	78.573064	73.577831
460.980112	87.496032	73.582836
460.602360	70.720172	73.587841
459.891701	71.740048	73.592846
459.468077	80.123806	73.597850
458.360696	83.534314	73.602855
457.585139	60.941773	73.607860
457.203170	76.441510	73.612865
456.848920	80.741218	73.617870
456.530315	76.616454	73.622874
455.165647	81.848213	73.627879
454.625962	71.467046	73.632884
454.112798	72.644682	73.637889
453.698597	90.183702	73.642894
452.785254	75.607722	73.647898
451.933755	80.667847	73.652903
451.311283	75.020954	73.657908
450.096421	97.258822	73.662913
449.891659	77.110900	73.667918
449.502774	57.544236	73.672922
448.762404	92.583034	73.677927
448.365914	80.848188	73.682932
447.432430	75.903660	73.687937
446.764738	78.444660	73.692942
446.515350	80.343468	73.697946
445.048935	90.845505	73.702951
444.355158	68.875401	73.707956
443.872969	74.915832	73.712961
443.236532	99.106723	73.717966
443.436272	65.968938	73.722970
441.813161	82.369690	73.727975
441.650872	59.477620	73.732980
441.056275	70.793163	73.737985
440.115550	73.201056	73.742990
439.303691	79.910560	73.747994
438.381322	73.001089	73.752999
438.031314	67.254028	73.758004
437.300013	72.634027	73.763009
436.921517	85.419465	73.768014
436.639926	77.017125	73.773018
435.206011	76.624271	73.778023
435.262535	83.097661	73.783028
434.088805	83.879105	73.788033
433.335997	72.609444	73.793038
432.686844	71.803000	73.798042
432.064596	78.269420	73.803047
432.065768	72.537365	73.808052
431.251263	73.476029	73.813057
430.167869	74.151625	73.818062
429.796109	73.067613	73.823066
428.778076	89.272636	73.828071
428.303577	78.819590	73.833076
427.446176	70.889015	73.838081
426.876979	79.530918	73.843086
426.534914	77.806706	73.848090
425.423056	76.097915	73.853095
424.895303	82.308026	73.858100
424.299539	78.260539	73.863105
423.834776	71.554116	73.868110
422.932540	78.642274	73.873114
422.020519	77.163402	73.878119
421.639499	67.975872	73.883124
421.433296	78.408006	73.888129
419.971137	80.414893	73.893134
419.244781	66.135556	73.898138
418.866768	89.350187	73.903143
418.723691	80.500030	73.908148
417.751370	71.906570	73.913153
416.772426	81.979310	73.918158
416.287437	78.865015	73.923162
415.749384	87.188170	73.928167
415.329942	80.824584	73.933172
414.446928	79.809417	73.938177
413.609082	78.101125	73.943182
413.042104	74.848517	73.948186
412.171872	80.351579	73.953191
411.408872	82.251805	73.958196
411.057340	81.385331	73.963201
410.409600	71.212195	73.968206
410.132748	77.880613	73.973210
409.015480	80.882735	73.978215
408.243820	84.848436	73.983220
407.740532	77.490608	73.988225
407.148407	86.517768	73.993230
406.453447	78.958681	73.998234
405.501794	89.675166	74.003239
405.102784	74.569437	74.008244
404.254614	81.202739	74.013249
403.903597	80.815547	74.018254
403.257694	87.615307	74.023258
402.228196	85.784600	74.028263
401.744327	77.359306	74.033268
401.458478	77.986681	74.038273
400.566082	74.087384	74.043278
399.832578	70.799817	74.048282
399.349872	76.635347	74.053287
398.887141	74.370585	74.058292
397.322241	80.965135	74.063297
396.694455	81.296933	74.068302
396.377264	78.941177	74.073306
395.708630	89.453307	74.078311
395.566896	79.838168	74.083316
395.192194	72.275365	74.088321
393.846179	80.979553	74.093326
393.602124	76.179069	74.098330
392.301474	81.430618	74.103335
391.283810	76.573639	74.108340
391.130027	69.215319	74.113345
390.473770	79.482636	74.118350
390.171044	74.934335	74.123354
389.474549	79.687525	74.128359
388.830102	72.073094	74.133364
388.023720	72.185787	74.138369
387.210157	72.105672	74.143374
386.389830	67.505817	74.148378
385.470156	81.697305	74.153383
384.919414	76.190379	74.158388
384.904208	69.418642	74.163393
384.401533	74.811107	74.168398
383.674032	71.181990	74.173402
382.453230	83.644357	74.178407
382.027661	70.718922	74.183412
381.569723	73.597073	74.188417
380.538264	77.455953	74.193422
380.237606	62.421300	74.198426
379.270626	76.943576	74.203431
378.961152	70.346453	74.208436
377.992217	81.690124	74.213441
377.244897	82.288539	74.218446
377.126272	73.395075	74.223450
375.952985	75.513641	74.228455
375.007265	64.025609	74.233460
374.540113	87.057330	74.238465
373.921267	81.390958	74.243470
374.161934	71.049465	74.248474
372.799802	79.871340	74.253479
372.045820	69.680457	74.258484
371.757011	68.733038	74.263489
370.331607	73.737987	74.268494
369.572776	74.609456	74.273498
368.703282	76.960296	74.278503
368.503512	81.459309	74.283508
368.578465	80.893864	74.288513
367.963773	73.900707	74.293518
367.432459	71.076062	74.298522
366.087462	83.585031	74.303527
365.564255	72.181048	74.308532
364.845295	74.235107	74.313537
363.475807	88.190798	74.318542
363.181898	77.762609	74.323546
362.564529	82.250901	74.328551
362.460308	67.557082	74.333556
362.445465	63.934252	74.338561
360.819773	75.884014	74.343566
360.309675	74.194473	74.348570
359.920944	80.655233	74.353575
358.584945	66.104089	74.358580
358.062224	79.860190	74.363585
357.045865	82.042063	74.368590
357.536210	74.959545	74.373594
356.435301	79.693613	74.378599
355.388066	76.974836	74.383604
355.077792	67.982617	74.388609
354.445752	78.753824	74.393614
353.296280	72.172299	74.398618
352.914224	84.553056	74.403623
352.381369	82.922331	74.408628
352.289761	84.829119	74.413633
350.630105	86.880133	74.418638
350.060078	77.579242	74.423642
349.590583	71.053353	74.428647
348.978203	79.156560	74.433652
348.456701	68.964908	74.438657
347.382244	76.815341	74.443662
346.955859	78.840127	74.448666
346.444979	78.415344	74.453671
345.834269	80.316550	74.458676
344.864729	72.014399	74.463681
344.125428	79.209070	74.468686
343.723844	76.904615	74.473690
343.363014	87.935366	74.478695
342.352788	79.764266	74.483700
341.375897	70.329538	74.488705
340.889504	80.839434	74.493710
340.773420	80.455810	74.498714
339.788397	87.052598	74.503719
338.872050	74.531790	74.508724
338.507031	79.621648	74.513729
337.625285	74.998484	74.518734
337.074326	77.506716	74.523738
335.930032	71.924095	74.528743
335.374544	76.383608	74.533748
335.203956	81.049847	74.538753
334.290928	88.163407	74.543758
334.377404	70.108900	74.548762
333.453276	84.204924	74.553767
332.968628	74.882550	74.558772
331.576423	81.906902	74.563777
330.452858	76.987985	74.568782
330.537711	65.081867	74.573786
330.094954	77.224727	74.578791
329.217234	77.662600	74.583796
328.394343	70.108166	74.588801
327.755427	74.257721	74.593806
327.329531	74.405985	74.598810
326.886234	76.307321	74.603815
326.072726	80.402706	74.608820
325.267987	69.989713	74.613825
324.500739	74.156566	74.618830
324.128541	70.492922	74.623834
323.136331	69.706489	74.628839
322.248203	72.446640	74.633844
321.804732	62.329293	74.638849
320.907539	75.126428	74.643854
320.791834	69.272669	74.648858
319.827322	79.474012	74.653863
318.982289	77.252848	74.658868
318.544187	70.094380	74.663873
317.996363	72.895409	74.668878
317.342219	71.889532	74.673882
316.286346	82.726716	74.678887
315.889321	73.642679	74.683892
315.515971	63.146753	74.688897
314.900039	75.635734	74.693902
313.900552	77.365532	74.698906
313.479062	79.518845	74.703911
312.783195	75.313891	74.708916
311.611172	75.145859	74.713921
310.647090	79.875484	74.718926
310.711465	78.058132	74.723930
309.957659	81.675684	74.728935
309.298713	70.779022	74.733940
309.302369	73.591504	74.738945
308.137601	83.397443	74.743950
307.750320	75.584370	74.748954
306.639039	83.123743	74.753959
305.890783	74.674387	74.758964
305.345075	70.656803	74.763969
304.839434	79.764801	74.768974
304.328981	65.405379	74.773978
303.106705	67.664240	74.778983
302.206357	79.277676	74.783988
302.159141	63.193472	74.788993
301.660763	71.158672	74.793998
300.956243	74.005177	74.799002
299.436948	82.150437	74.804007
299.093501	69.483159	74.809012
299.296750	59.035684	74.814017
298.405065	72.328650	74.819022
297.417691	68.196969	74.824026
296.826096	74.699525	74.829031
296.209670	78.224226	74.834036
295.808137	64.989085	74.839041
294.477683	75.012229	74.844046
294.309778	62.157720	74.849050
293.396436	71.403227	74.854055
292.716526	70.248509	74.859060
291.971147	69.864266	74.864065
291.231571	74.228554	74.869070
290.873660	69.976053	74.874074
290.491657	61.626023	74.879079
289.638562	75.594040	74.884084
289.054886	77.531948	74.889089
288.262848	77.744881	74.894094
287.975511	66.230801	74.899098
286.893562	72.639635	74.904103
286.201802	75.955587	74.909108
285.898379	72.828153	74.914113
284.418955	79.877466	74.919118
283.927962	71.831788	74.924122
283.139479	80.239021	74.929127
282.536394	74.718392	74.934132
282.725123	69.010067	74.939137
281.967239	81.507489	74.944142
281.336317	65.270332	74.949146
280.575504	73.605347	74.954151
279.724617	75.711993	74.959156
278.576514	70.502145	74.964161
277.854672	89.938255	74.969166
277.390969	79.950281	74.974170
277.062891	74.839953	74.979175
276.657917	76.750958	74.984180
275.709887	71.075591	74.989185
274.728067	73.548436	74.994190
274.457897	74.206439	74.999194
273.926747	82.774496	75.004199
272.912515	71.638029	75.009204
272.325508	70.121604	75.014209
271.656154	65.439388	75.019214
271.358403	68.530127	75.024218
270.280443	72.789092	75.029223
269.280850	70.269329	75.034228
269.153327	76.240639	75.039233
268.655942	76.736175	75.044238
267.947294	68.881303	75.049242
267.118793	69.175744	75.054247
266.473334	73.843560	75.059252
265.795830	71.713977	75.064257
264.415163	78.315503	75.069262
263.768599	77.297395	75.074266
263.228144	80.346402	75.079271
262.612722	73.974673	75.084276
262.595679	71.244691	75.089281
262.059330	75.459908	75.094286
261.800711	72.186575	75.099290
260.984891	70.547362	75.104295
260.215040	74.301515	75.109300
259.287858	75.348074	75.114305
258.013780	84.151237	75.119310
257.979659	66.705710	75.124314
257.214073	76.325043	75.129319
256.505514	85.648307	75.134324
255.608693	75.174329	75.139329
254.926374	77.963695	75.144334
254.899440	73.000900	75.149338
254.003749	73.132602	75.154343
252.855991	80.039186	75.159348
252.278228	76.952332	75.164353
251.747922	92.985047	75.169358
251.364445	78.431940	75.174362
250.919736	66.867264	75.179367
249.995801	80.312035	75.184372
249.563750	70.486176	75.189377
248.716716	80.586819	75.194382
247.787807	62.233746	75.199386
247.132764	69.265203	75.204391
246.617047	70.604124	75.209396
246.472393	68.124703	75.214401
244.929277	82.557512	75.219406
244.562863	68.011158	75.224410
243.828180	64.130940	75.229415
243.340340	72.447681	75.234420
242.792417	64.800574	75.239425
241.822488	68.075725	75.244430
241.068895	71.962899	75.249434
240.752730	68.619900	75.254439
240.053756	75.852316	75.259444
239.338423	77.130023	75.264449
238.610567	70.329978	75.269454
238.186820	62.735615	75.274458
237.343441	62.490004	75.279463
236.298006	69.541117	75.284468
235.663403	59.217737	75.289473
235.377882	66.037338	75.294478
235.149106	54.521830	75.299482
234.209979	54.256792	75.304487
233.518778	62.061933	75.309492
233.131774	70.152880	75.314497
231.722239	69.355742	75.319502
230.885158	60.859086	75.324506
230.074104	65.816636	75.329511
230.139832	72.960270	75.334516
229.711835	64.469361	75.339521
229.113521	77.917419	75.344526
228.557007	69.849089	75.349530
227.696234	67.764500	75.354535
226.869667	69.201858	75.359540
225.869914	71.111492	75.364545
225.163171	75.475294	75.369550
224.481943	69.472012	75.374554
224.034570	70.691241	75.379559
223.753572	64.545320	75.384564
223.253235	69.773442	75.389569
221.985184	77.347295	75.394574
221.615062	77.125589	75.399578
221.099813	68.066734	75.404583
219.719604	75.909184	75.409588
219.413802	58.172692	75.414593
218.758260	69.862226	75.419598
218.385285	70.287481	75.424602
217.444600	71.333054	75.429607
216.681952	71.933960	75.434612
216.237419	72.578766	75.439617
215.483978	72.768226	75.444622
215.531441	63.305881	75.449626
214.474782	70.409251	75.454631
213.429926	67.020003	75.459636
213.218609	70.918504	75.464641
211.808201	65.619630	75.469646
211.283415	72.299193	75.474650
210.650240	62.456530	75.479655
210.050557	87.944013	75.484660
210.231512	66.809084	75.489665
209.013393	70.232613	75.494670
207.621549	83.599033	75.499674
207.733028	66.899806	75.504679
207.230040	75.004516	75.509684
206.816664	81.361993	75.514689
205.839171	76.825103	75.519694
205.275247	71.526899	75.524698
204.147824	71.623026	75.529703
203.158333	66.851526	75.534708
202.653316	65.761989	75.539713
202.158335	74.060951	75.544718
201.824703	67.816198	75.549722
201.423995	68.529709	75.554727
200.413440	79.720799	75.559732
200.211125	74.929459	75.564737
199.290629	70.172191	75.569742
198.274347	70.392519	75.574746
197.513293	71.206050	75.579751
196.823185	73.955673	75.584756
196.969887	76.415787	75.589761
195.397871	81.411089	75.594766
194.807100	78.744188	75.599770
194.498011	75.914118	75.604775
193.813970	79.331357	75.609780
193.640226	69.379187	75.614785
192.279547	62.817231	75.619790
191.803826	85.022460	75.624794
191.567099	70.919038	75.629799
190.145552	80.390666	75.634804
189.754264	79.178928	75.639809
188.879687	77.493917	75.644814
188.473968	73.566003	75.649818
188.137237	74.527918	75.654823
186.677795	82.460284	75.659828
186.497466	68.977035	75.664833
186.037393	76.109879	75.669838
185.574504	70.300444	75.674842
184.422703	68.249653	75.679847
183.701000	82.092678	75.684852
183.341306	67.463277	75.689857
182.424852	80.118449	75.694862
181.582254	69.394610	75.699866
181.171207	78.490693	75.704871
180.685629	72.662800	75.709876
180.377623	71.929762	75.714881
179.226761	72.212551	75.719886
178.731449	76.227288	75.724890
177.893096	75.088403	75.729895
177.016470	74.168493	75.734900
175.971343	80.245094	75.739905
175.484594	67.616466	75.744910
174.856587	68.643743	75.749914
174.534039	77.673681	75.754919
173.966298	73.445193	75.759924
173.837097	61.196355	75.764929
172.974922	81.446408	75.769934
172.210460	72.892465	75.774938
171.304796	69.317054	75.779943
170.202698	63.442389	75.784948
169.740198	65.733136	75.789953
169.078602	72.213759	75.794958
168.827906	74.423435	75.799962
168.445844	74.079071	75.804967
167.603343	84.240509	75.809972
166.823169	77.415715	75.814977
166.083479	70.716924	75.819982
165.095293	70.548037	75.824986
164.501842	77.065104	75.829991
163.969793	82.741388	75.834996
163.821270	70.284327	75.840001
162.749411	75.229866	75.845006
161.637194	78.650727	75.850010
161.336095	72.438638	75.855015
160.586213	83.687524	75.860020
160.316489	75.418959	75.865025
159.802063	77.773178	75.870030
158.536067	74.548512	75.875034
158.349637	74.057849	75.880039
157.058305	82.203107	75.885044
156.536722	76.983314	75.890049
155.823190	86.050364	75.895054
155.306301	78.642740	75.900058
155.154712	69.617382	75.905063
154.576459	72.839579	75.910068
153.503943	73.978729	75.915073
152.504406	75.172472	75.920078
151.933474	72.237510	75.925082
151.655416	71.706268	75.930087
150.823142	87.427605	75.935092
150.276384	73.685836	75.940097
149.568277	85.645528	75.945102
149.102314	84.688536	75.950106
148.066372	85.787168	75.955111
147.344274	84.549338	75.960116
146.866781	77.723598	75.965121
146.358643	85.378165	75.970126
145.450164	80.191676	75.975130
144.469546	79.851291	75.980135
143.779340	90.543506	75.985140
143.736628	80.029588	75.990145
143.218460	79.547667	75.995150
142.334508	83.933438	76.000154
141.723738	82.435026	76.005159
141.059081	70.413475	76.010164
140.901995	70.971465	76.015169
139.468011	74.303298	76.020174
138.698680	80.797954	76.025178
138.675482	86.191276	76.030183
137.165079	83.682054	76.035188
136.694571	77.388176	76.040193
136.106001	84.076349	76.045198
135.562289	78.103204	76.050202
135.328628	68.114870	76.055207
134.214069	80.350663	76.060212
133.793201	82.426638	76.065217
132.887690	85.164895	76.070222
132.480409	83.865836	76.075226
131.520494	80.568728	76.080231
130.824485	86.636988	76.085236
130.443597	87.139207	76.090241
130.107593	81.080910	76.095246
129.301139	83.691418	76.100250
128.481910	78.631045	76.105255
127.315421	81.158620	76.110260
127.366791	80.480244	76.115265
125.905969	71.859169	76.120270
125.054165	83.009202	76.125274
124.782555	72.795122	76.130279
124.116849	84.614025	76.135284
123.886633	69.438907	76.140289
123.603951	79.690851	76.145294
122.685088	79.416317	76.150298
122.171997	75.054558	76.155303
121.096826	84.303847	76.160308
119.993095	72.940475	76.165313
119.610167	81.497531	76.170318
119.159171	77.685651	76.175322
119.034532	77.041646	76.180327
117.739462	86.518375	76.185332
117.184692	67.924378	76.190337
116.315847	81.633190	76.195342
115.905861	82.053324	76.200346
115.119005	74.759718	76.205351
114.165932	79.719451	76.210356
113.578608	78.526369	76.215361
113.243850	74.333283	76.220366
113.028775	75.564373	76.225370
112.120617	71.470602	76.230375
111.278596	75.304107	76.235380
110.973886	73.510915	76.240385
109.796943	93.341284	76.245390
109.163467	94.528711	76.250394
109.146904	70.217988	76.255399
107.498410	94.382599	76.260404
107.014990	80.785270	76.265409
106.320065	75.577363	76.270414
106.040491	83.633850	76.275418
105.682463	85.239371	76.280423
104.563732	72.229023	76.285428
104.130650	68.382755	76.290433
103.152076	76.470279	76.295438
102.526291	85.712569	76.300442
101.942528	79.203386	76.305447
100.773942	87.721733	76.310452
100.432937	72.157458	76.315457
100.044197	95.747487	76.320462
99.607739	81.067265	76.325466
98.656198	88.789389	76.330471
97.746334	81.288336	76.335476
97.367218	100.136850	76.340481
96.824475	70.824710	76.345486
96.231086	86.310858	76.350490
95.488513	77.215750	76.355495
94.698537	83.436186	76.360500
94.356566	76.730767	76.365505
93.084001	73.360539	76.370510
92.476188	78.784004	76.375514
92.090365	67.276215	76.380519
91.610472	84.049887	76.385524
90.767022	69.362044	76.390529
90.097905	75.550591	76.395534
89.399281	82.226359	76.400538
89.008455	73.399996	76.405543
87.753047	80.965585	76.410548
87.225393	66.936968	76.415553
86.639492	76.056208	76.420558
86.235433	62.722196	76.425562
85.279910	72.937935	76.430567
84.264195	79.776224	76.435572
84.012636	62.652397	76.440577
83.692853	93.620499	76.445582
82.762022	60.309903	76.450586
82.206797	84.401088	76.455591
81.036453	79.879238	76.460596
80.699054	85.954974	76.465601
80.740684	85.267112	76.470606
79.457840	73.102906	76.475610
78.689145	70.563751	76.480615
77.998574	103.210416	76.485620
77.809709	70.959384	76.490625
77.134757	92.229785	76.495630
76.127018	84.621353	76.500634
75.561761	77.275079	76.505639
75.049352	80.759588	76.510644
73.926690	76.561275	76.515649
73.046167	73.998957	76.520654
72.545551	96.477806	76.525658
72.639636	77.725156	76.530663
71.767101	80.268953	76.535668
70.806766	77.053935	76.540673
70.397619	76.417459	76.545678
69.345889	80.267075	76.550682
69.180738	82.119367	76.555687
68.635741	73.601426	76.560692
67.746975	70.072244	76.565697
67.210809	92.400649	76.570702
66.249402	74.893306	76.575706
65.473788	70.672770	76.580711
64.787222	77.699831	76.585716
64.375979	75.355972	76.590721
64.030578	75.196575	76.595726
62.875402	73.731389	76.600730
62.263204	73.728072	76.605735
61.377183	75.930272	76.610740
61.132358	67.097982	76.615745
60.340064	64.860621	76.620750
59.509496	69.036064	76.625754
58.958265	66.340820	76.630759
58.352856	72.046160	76.635764
57.577552	67.426638	76.640769
56.520847	70.371943	76.645774
56.041336	69.565355	76.650778
55.801806	73.603971	76.655783
55.225069	71.504109	76.660788
55.029930	61.096521	76.665793
53.958344	57.143951	76.670798
53.006384	67.228249	76.675802
52.483668	69.266864	76.680807
51.329145	71.880867	76.685812
51.081248	76.327643	76.690817
50.621701	63.723106	76.695822
49.750211	71.046144	76.700826
49.098160	59.062051	76.705831
47.928386	75.002784	76.710836
47.463413	64.496311	76.715841
47.613738	58.754691	76.720846
47.060662	72.441533	76.725850
46.176458	62.221102	76.730855
45.323978	70.258571	76.735860
44.426129	61.082609	76.740865
43.279027	56.243289	76.745870
42.571402	69.563720	76.750874
42.525537	61.429784	76.755879
41.593219	66.438262	76.760884
41.430760	66.721168	76.765889
40.781988	65.794931	76.770894
39.926024	69.340541	76.775898
39.319454	72.024845	76.780903
38.459546	66.824353	76.785908
38.157627	53.691679	76.790913
37.143685	64.533287	76.795918
36.198096	68.831152	76.800922
36.317772	70.213849	76.805927
35.201064	69.776950	76.810932
34.226148	66.956908	76.815937
33.531546	71.672031	76.820942
33.502012	67.040804	76.825946
33.131183	58.870394	76.830951
31.756849	74.295015	76.835956
30.734208	66.465082	76.840961
30.290804	60.211068	76.845966
29.926887	69.823150	76.850970
29.767761	60.165130	76.855975
28.677517	72.516912	76.860980
28.250584	72.015735	76.865985
27.440705	62.343237	76.870990
26.316951	62.874068	76.875994
25.798920	60.432141	76.880999
25.354014	66.301107	76.886004
24.978236	59.525415	76.891009
24.196209	66.621316	76.896014
22.999652	70.678535	76.901018
22.693810	63.544782	76.906023
22.565935	70.399171	76.911028
21.693708	72.980779	76.916033
20.730111	62.985895	76.921038
19.840437	61.325434	76.926042
19.561431	57.744753	76.931047
18.317419	69.920802	76.936052
17.746391	66.790365	76.941057
17.395928	68.347384	76.946062
17.032601	69.751924	76.951066
16.633544	57.766916	76.956071
15.098274	66.826279	76.961076
14.872845	58.205361	76.966081
14.500277	58.889182	76.971086
13.125675	67.648552	76.976090
12.498511	52.612479	76.981095
11.836268	63.721252	76.986100
11.608489	56.213958	76.991105
11.362035	62.270454	76.996110
9.979249	74.884929	77.001114
9.450061	66.118503	77.006119
8.702373	75.343975	77.011124
8.101917	67.755777	77.016129
7.340492	75.709355	77.021134
6.278815	68.385517	77.026139
5.930440	70.508290	77.031143
5.772232	76.694210	77.036148
5.147217	73.189213	77.041153
4.435853	60.563361	77.046158