Mon Mar 08 20:22:58 2021

Number of Points = 14582

Depth (nm)	Load (N)	Time (s)
-0.861822	105.229803	0.000000
-1.366756	104.588167	0.005005
-1.903436	57.551501	0.010010
-4.158380	25.724849	0.015014
-8.870526	23.157309	0.020019
-14.301802	24.430555	0.025024
-18.960487	27.313506	0.030029
-23.010916	20.539089	0.035034
-27.035388	27.387534	0.040038
-30.889561	29.150336	0.045043
-34.018181	27.418240	0.050048
-38.151258	36.155733	0.055053
-41.640133	24.755209	0.060058
-45.242323	36.741445	0.065062
-49.257022	29.821031	0.070067
-52.691475	18.608951	0.075072
-56.866480	31.661067	0.080077
-60.219578	21.385271	0.085082
-64.227196	30.197397	0.090086
-68.424167	28.027138	0.095091
-71.880996	25.727761	0.100096
-75.305221	29.361540	0.105101
-79.231680	20.162773	0.110106
-83.022658	25.408257	0.115110
-86.909818	29.379245	0.120115
-90.284272	24.428711	0.125120
-93.811416	27.758839	0.130125
-97.792353	18.559336	0.135130
-101.957082	23.135987	0.140134
-106.026752	15.097016	0.145139
-109.822533	18.993537	0.150144
-113.967392	27.157484	0.155149
-117.345388	23.733928	0.160154
-120.955195	19.778132	0.165158
-124.694357	19.469694	0.170163
-128.083674	16.459515	0.175168
-132.299569	25.246636	0.180173
-135.941422	18.982765	0.185178
-139.587438	16.731023	0.190182
-143.193301	24.900462	0.195187
-146.600514	17.864361	0.200192
-150.733514	23.320632	0.205197
-154.465464	28.096370	0.210202
-158.337449	22.119974	0.215206
-162.278189	29.789415	0.220211
-165.695628	20.623097	0.225216
-169.747670	29.354174	0.230221
-173.383466	35.120616	0.235226
-176.934438	21.596763	0.240230
-180.811075	23.686636	0.245235
-184.778891	29.296362	0.250240
-188.690294	26.820563	0.255245
-192.041792	14.387610	0.260250
-196.139528	27.427612	0.265254
-200.095128	32.395220	0.270259
-203.424330	24.613524	0.275264
-207.408014	22.231288	0.280269
-210.842977	27.948383	0.285274
-214.245799	20.635736	0.290278
-218.462341	29.744778	0.295283
-222.328287	19.970518	0.300288
-226.573604	32.647803	0.305293
-229.681347	30.933131	0.310298
-233.408389	25.592839	0.315302
-237.378700	22.724432	0.320307
-240.982499	25.762677	0.325312
-245.145395	24.730493	0.330317
-248.829564	21.253504	0.335322
-252.124949	13.135354	0.340326
-256.251652	12.929979	0.345331
-260.093667	16.381560	0.350336
-264.007976	19.314874	0.355341
-267.511063	26.424222	0.360346
-271.041836	27.864564	0.365350
-275.069547	25.546236	0.370355
-278.601473	25.372100	0.375360
-282.303254	31.660124	0.380365
-286.396027	19.467060	0.385370
-290.032829	21.928795	0.390374
-294.033347	22.165352	0.395379
-297.407316	35.686018	0.400384
-300.970879	26.827058	0.405389
-304.745327	18.077465	0.410394
-308.797801	25.492178	0.415398
-312.820330	24.456625	0.420403
-316.209652	24.031138	0.425408
-320.339002	35.840154	0.430413
-324.006412	27.368365	0.435418
-327.858904	25.269715	0.440422
-331.470702	29.567679	0.445427
-335.166364	21.538781	0.450432
-339.200566	30.871204	0.455437
-342.567587	29.533940	0.460442
-346.238172	28.057507	0.465446
-350.289307	35.420042	0.470451
-353.785754	22.557923	0.475456
-357.864692	32.018935	0.480461
-361.706829	21.887902	0.485466
-365.767856	21.725841	0.490470
-369.092470	26.944601	0.495475
-372.700027	22.898954	0.500480
-376.104728	34.707460	0.505485
-380.339756	32.113354	0.510490
-384.191239	27.375025	0.515494
-387.951585	32.780072	0.520499
-391.607199	26.491994	0.525504
-395.294844	29.740958	0.530509
-399.121139	24.224410	0.535514
-402.966512	28.212875	0.540518
-407.008487	34.192737	0.545523
-410.508267	20.162815	0.550528
-414.413181	20.685479	0.555533
-418.029716	24.836104	0.560538
-421.300649	22.942757	0.565542
-425.244341	30.117956	0.570547
-429.228034	33.256566	0.575552
-432.938573	23.905667	0.580557
-436.994054	30.988359	0.585562
-440.674854	33.182979	0.590566
-444.622300	26.157908	0.595571
-447.974862	21.779943	0.600576
-451.684954	29.699982	0.605581
-455.508399	23.642221	0.610586
-458.879735	21.239879	0.615590
-463.499459	23.581332	0.620595
-467.005242	12.433329	0.625600
-470.849381	21.306704	0.630605
-474.086413	23.895661	0.635610
-477.927587	22.484522	0.640614
-482.053611	28.566231	0.645619
-485.404038	22.442433	0.650624
-489.808751	25.676768	0.655629
-493.473241	25.022693	0.660634
-496.791154	34.885883	0.665638
-500.794515	38.188588	0.670643
-504.315525	27.216516	0.675648
-508.355895	25.830935	0.680653
-511.895832	27.960589	0.685658
-515.413213	25.400320	0.690662
-519.724507	19.447400	0.695667
-523.203844	20.685945	0.700672
-527.113838	26.783679	0.705677
-531.024062	29.745153	0.710682
-534.607435	28.974113	0.715686
-538.480180	30.493125	0.720691
-541.994349	26.622042	0.725696
-545.789908	36.184734	0.730701
-549.852034	28.203687	0.735706
-553.270488	30.091662	0.740710
-557.162355	33.337229	0.745715
-560.921547	20.250936	0.750720
-564.732151	30.246529	0.755725
-568.691321	30.916874	0.760730
-572.134380	26.865756	0.765734
-576.281706	23.406511	0.770739
-579.454639	8.675008	0.775744
-583.160471	25.695976	0.780749
-587.246132	30.749631	0.785754
-590.903714	22.650418	0.790758
-594.983782	23.272317	0.795763
-598.827333	21.207374	0.800768
-602.392264	18.596493	0.805773
-605.930193	32.634132	0.810778
-609.442183	7.519852	0.815782
-613.468019	24.587258	0.820787
-617.187867	20.370715	0.825792
-621.273610	35.754209	0.830797
-624.745451	23.732196	0.835802
-628.656329	27.340429	0.840806
-632.575575	27.933543	0.845811
-636.256129	21.205182	0.850816
-640.066040	28.679438	0.855821
-644.148423	30.315689	0.860826
-647.572074	24.378857	0.865830
-651.340512	33.024392	0.870835
-654.545367	23.108976	0.875840
-658.380811	22.482473	0.880845
-662.167148	30.651529	0.885850
-665.853431	22.918117	0.890854
-670.347049	28.686750	0.895859
-673.790075	27.541863	0.900864
-677.499346	27.071833	0.905869
-681.445370	22.913613	0.910874
-685.025034	25.390462	0.915878
-688.977148	23.491236	0.920883
-692.536231	23.180141	0.925888
-696.382653	23.840564	0.930893
-700.308548	24.253518	0.935898
-703.901005	16.405839	0.940902
-707.687931	21.424565	0.945907
-711.210539	15.465805	0.950912
-714.873696	24.895630	0.955917
-718.647278	27.278951	0.960922
-722.369477	21.539745	0.965926
-726.204255	23.016726	0.970931
-730.272454	26.889942	0.975936
-734.171384	28.307809	0.980941
-737.746361	17.399934	0.985946
-741.604244	21.644797	0.990950
-745.917612	34.131978	0.995955
-749.023982	22.605217	1.000960
-752.883224	19.671054	1.005965
-756.676534	30.480964	1.010970
-760.026628	29.950502	1.015974
-763.847086	26.100331	1.020979
-767.382484	32.135420	1.025984
-771.649053	32.382190	1.030989
-775.603043	28.889244	1.035994
-779.119198	12.364866	1.040998
-783.167570	22.933329	1.046003
-786.553238	27.358229	1.051008
-790.335650	17.089097	1.056013
-794.227983	30.836738	1.061018
-797.631317	24.669824	1.066022
-801.769208	31.515570	1.071027
-805.278295	22.465801	1.076032
-809.392625	31.799169	1.081037
-813.193081	35.274942	1.086042
-816.575010	31.597586	1.091046
-820.446584	32.188121	1.096051
-824.277094	23.175573	1.101056
-827.962222	26.960910	1.106061
-831.670623	39.345221	1.111066
-835.580060	23.631209	1.116070
-839.456710	24.265161	1.121075
-843.024481	16.721239	1.126080
-846.993132	32.742319	1.131085
-850.945645	33.033633	1.136090
-854.339398	23.208630	1.141094
-858.487314	26.121910	1.146099
-861.702649	13.242486	1.151104
-865.704909	29.879192	1.156109
-869.474890	22.667234	1.161114
-873.256851	20.372143	1.166118
-876.580958	20.512571	1.171123
-880.102893	8.498991	1.176128
-884.032825	16.375971	1.181133
-888.190004	21.402142	1.186138
-891.838366	17.411140	1.191142
-895.840968	26.266351	1.196147
-899.356149	19.464675	1.201152
-903.149910	24.224624	1.206157
-906.973173	20.241113	1.211162
-910.958162	18.982980	1.216166
-914.674620	24.126367	1.221171
-918.292664	18.012894	1.226176
-922.012755	13.148817	1.231181
-925.632595	16.170143	1.236186
-929.298362	18.270074	1.241190
-933.359041	26.773542	1.246195
-936.948123	19.017154	1.251200
-940.695839	15.430015	1.256205
-944.986301	23.017848	1.261210
-948.588613	11.450856	1.266214
-952.364249	10.495178	1.271219
-955.753625	16.472491	1.276224
-959.717410	21.978746	1.281229
-963.278122	29.632824	1.286234
-966.961494	16.226061	1.291238
-971.027523	24.940162	1.296243
-974.647892	19.945114	1.301248
-978.429972	23.854985	1.306253
-982.182184	19.220050	1.311258
-985.859256	22.688976	1.316262
-989.555573	12.857392	1.321267
-993.450267	18.809927	1.326272
-997.509728	26.181152	1.331277
-1001.379391	26.243446	1.336282
-1004.936683	24.420371	1.341286
-1008.603562	29.287916	1.346291
-1012.320432	16.309176	1.351296
-1016.049211	23.977594	1.356301
-1019.963624	17.228926	1.361306
-1023.361794	23.475800	1.366310
-1027.414834	18.937938	1.371315
-1030.965730	18.288609	1.376320
-1034.860066	24.435104	1.381325
-1038.697560	26.201581	1.386330
-1042.148616	22.056268	1.391334
-1046.371193	24.567115	1.396339
-1049.755540	25.565752	1.401344
-1053.433887	32.761003	1.406349
-1057.620654	25.409468	1.411354
-1061.349664	26.956797	1.416358
-1065.196506	30.733676	1.421363
-1068.814640	22.841811	1.426368
-1072.533374	17.846888	1.431373
-1076.386606	17.225494	1.436378
-1079.931197	20.088373	1.441382
-1084.088595	25.565886	1.446387
-1087.368409	25.486659	1.451392
-1091.074082	19.792724	1.456397
-1094.808844	13.321352	1.461402
-1098.762154	15.722988	1.466406
-1102.916253	23.235671	1.471411
-1106.391803	16.317607	1.476416
-1109.930461	23.651426	1.481421
-1113.991034	27.495690	1.486426
-1117.407528	15.508199	1.491430
-1121.677889	23.727005	1.496435
-1125.205798	37.330123	1.501440
-1128.407055	19.614331	1.506445
-1132.824921	18.351726	1.511450
-1136.599652	12.306252	1.516454
-1140.551744	20.956673	1.521459
-1143.757459	31.274217	1.526464
-1147.591094	27.412606	1.531469
-1151.577531	22.954186	1.536474
-1155.335177	16.210634	1.541478
-1158.720194	42.172075	1.546483
-1162.655761	9.822744	1.551488
-1166.731800	31.197421	1.556493
-1170.530920	42.997553	1.561498
-1173.981856	18.678665	1.566502
-1177.689273	29.272053	1.571507
-1181.256511	10.027068	1.576512
-1184.960953	21.307475	1.581517
-1189.424924	26.078933	1.586522
-1193.128115	18.811112	1.591526
-1196.881290	27.871304	1.596531
-1200.299836	18.810837	1.601536
-1203.730786	11.668192	1.606541
-1207.718084	8.818362	1.611546
-1211.610737	29.302819	1.616550
-1215.580044	36.045027	1.621555
-1219.447949	25.482836	1.626560
-1222.857609	20.921205	1.631565
-1226.535123	13.944197	1.636570
-1229.853111	10.556824	1.641574
-1234.156194	31.673076	1.646579
-1238.610894	25.082211	1.651584
-1242.151850	27.020741	1.656589
-1245.771479	21.923518	1.661594
-1248.924218	8.345604	1.666598
-1253.002959	34.456011	1.671603
-1256.674099	32.547477	1.676608
-1260.305827	23.339887	1.681613
-1264.509252	36.010613	1.686618
-1267.872301	27.108507	1.691622
-1271.820827	22.108118	1.696627
-1275.527354	10.271376	1.701632
-1279.173587	12.948989	1.706637
-1283.183164	14.740254	1.711642
-1287.076982	25.997515	1.716646
-1290.658670	24.937235	1.721651
-1294.520260	21.734726	1.726656
-1298.248314	13.179657	1.731661
-1302.006081	21.876497	1.736666
-1305.598491	19.499744	1.741670
-1309.700852	29.562088	1.746675
-1312.958820	15.143324	1.751680
-1316.760719	20.939614	1.756685
-1320.898781	17.642648	1.761690
-1324.331957	4.377801	1.766694
-1328.308036	30.506567	1.771699
-1332.050920	21.682713	1.776704
-1335.728243	25.420278	1.781709
-1339.848588	25.389236	1.786714
-1343.357839	6.759675	1.791718
-1346.889347	40.220431	1.796723
-1350.440684	11.594324	1.801728
-1354.693941	29.131321	1.806733
-1358.434252	27.339672	1.811738
-1362.238938	11.557848	1.816742
-1366.020642	32.765873	1.821747
-1369.557484	23.082847	1.826752
-1373.229304	21.393789	1.831757
-1377.158045	26.740595	1.836762
-1380.517699	18.572920	1.841766
-1384.364906	18.485614	1.846771
-1388.561080	12.000310	1.851776
-1392.331274	23.059760	1.856781
-1396.341850	12.523893	1.861786
-1399.469619	17.941170	1.866790
-1403.719118	33.560252	1.871795
-1407.054564	18.945899	1.876800
-1410.851994	19.943396	1.881805
-1414.911621	31.246329	1.886810
-1418.714116	24.510402	1.891814
-1422.460876	22.093898	1.896819
-1426.297328	23.476103	1.901824
-1429.713133	21.124880	1.906829
-1433.535281	33.941400	1.911834
-1437.086688	31.075784	1.916838
-1440.908139	28.623966	1.921843
-1444.963960	19.889837	1.926848
-1448.710635	31.907466	1.931853
-1452.741760	33.462800	1.936858
-1455.989840	13.460777	1.941862
-1459.942776	20.654879	1.946867
-1463.536350	36.739833	1.951872
-1467.400637	24.015705	1.956877
-1471.041137	18.125905	1.961882
-1474.812936	17.255616	1.966886
-1478.864170	36.026650	1.971891
-1482.623340	27.303422	1.976896
-1486.144000	13.969271	1.981901
-1490.123452	30.065594	1.986906
-1493.494319	25.390940	1.991910
-1497.531377	0.573644	1.996915
-1501.291421	27.729595	2.006912
-1502.437466	19.430128	2.016909
-1499.867166	25.618006	2.026906
-1497.110846	18.412912	2.036902
-1494.989467	11.547913	2.046899
-1493.182722	30.918128	2.056896
-1491.099216	14.747278	2.066893
-1489.355367	22.632137	2.076890
-1487.309373	17.247523	2.086886
-1485.290801	21.886530	2.096883
-1483.504886	20.812715	2.106880
-1481.650195	22.449783	2.116877
-1480.020835	27.902649	2.126874
-1477.860543	19.610485	2.136870
-1475.826196	29.733400	2.146867
-1474.107926	24.478639	2.156864
-1472.172049	30.854983	2.166861
-1470.226706	30.222980	2.176858
-1468.337859	27.782795	2.186854
-1466.549163	28.944166	2.196851
-1464.771225	30.653536	2.206848
-1462.372452	34.344384	2.216845
-1460.689422	32.966559	2.226842
-1459.056285	28.262241	2.236838
-1457.074604	25.121989	2.246835
-1455.312476	33.987565	2.256832
-1453.195055	33.001203	2.266829
-1451.249372	28.665231	2.276826
-1449.528347	28.261782	2.286822
-1447.768257	19.729014	2.296819
-1445.567857	30.491634	2.306816
-1443.800909	28.663049	2.316813
-1442.099025	30.690907	2.326810
-1439.922882	29.766202	2.336806
-1438.237068	24.636654	2.346803
-1436.371476	25.375240	2.356800
-1434.438620	25.083135	2.366797
-1432.559395	31.983286	2.376794
-1430.805824	26.405557	2.386790
-1428.631909	18.224930	2.396787
-1427.013812	11.437416	2.406784
-1425.017648	24.803086	2.416781
-1423.254109	26.156399	2.426778
-1421.294494	24.518017	2.436774
-1419.285793	26.321516	2.446771
-1417.402779	30.263929	2.456768
-1415.688888	26.806615	2.466765
-1413.937783	24.115391	2.476762
-1411.914427	28.199535	2.486758
-1410.033412	25.620135	2.496755
-1408.057094	22.082918	2.506752
-1406.232045	25.398352	2.516749
-1404.300915	23.581401	2.526746
-1402.387538	26.832174	2.536742
-1400.646895	29.341716	2.546739
-1398.832589	29.655946	2.556736
-1396.853790	32.354713	2.566733
-1394.995648	34.397061	2.576730
-1393.022381	24.909738	2.586726
-1391.325035	26.374719	2.596723
-1389.012291	19.171297	2.606720
-1387.536971	31.385756	2.616717
-1385.615678	32.762787	2.626714
-1383.968515	24.118675	2.636710
-1381.857585	25.108532	2.646707
-1379.581938	22.113897	2.656704
-1378.195149	31.284348	2.666701
-1376.291158	27.493492	2.676698
-1374.168890	32.168107	2.686694
-1372.415474	30.516991	2.696691
-1370.729110	27.171476	2.706688
-1368.658877	28.171018	2.716685
-1366.652212	31.932638	2.726682
-1365.106257	31.138890	2.736678
-1363.246262	28.670252	2.746675
-1361.009180	34.785338	2.756672
-1359.383348	28.566578	2.766669
-1357.260798	27.178460	2.776666
-1355.384800	28.603817	2.786662
-1353.572623	28.293207	2.796659
-1351.958669	34.140190	2.806656
-1350.052988	29.619664	2.816653
-1347.768273	27.150937	2.826650
-1346.331833	29.725008	2.836646
-1344.283825	28.544610	2.846643
-1342.128890	27.118166	2.856640
-1340.423767	23.943341	2.866637
-1338.776397	30.490719	2.876634
-1336.906702	22.437810	2.886630
-1334.748653	21.351901	2.896627
-1333.006685	23.305535	2.906624
-1331.136128	27.455263	2.916621
-1329.623597	29.338268	2.926618
-1327.288078	31.942102	2.936614
-1325.334378	29.422180	2.946611
-1323.305574	34.762285	2.956608
-1321.722066	30.185992	2.966605
-1320.077797	28.435553	2.976602
-1317.808394	31.766769	2.986598
-1316.152535	22.264003	2.996595
-1314.418468	20.775490	3.006592
-1312.416987	25.221621	3.016589
-1310.461526	30.118772	3.026586
-1308.348169	23.259946	3.036582
-1306.560414	36.676474	3.046579
-1304.777246	25.460829	3.056576
-1303.194623	31.098142	3.066573
-1301.209582	31.538267	3.076570
-1299.119457	29.711740	3.086566
-1297.401881	30.463081	3.096563
-1295.162969	19.809187	3.106560
-1293.503656	22.560760	3.116557
-1291.932116	25.749511	3.126554
-1289.779303	21.625235	3.136550
-1287.816961	26.372894	3.146547
-1286.059199	23.649122	3.156544
-1284.373060	28.515199	3.166541
-1282.096215	25.217329	3.176538
-1280.470672	25.876053	3.186534
-1278.571646	30.678063	3.196531
-1277.023790	26.244864	3.206528
-1274.623023	19.090612	3.216525
-1272.825248	29.017926	3.226522
-1271.004252	25.699876	3.236518
-1269.029005	28.381957	3.246515
-1267.267331	23.783500	3.256512
-1265.560842	28.622652	3.266509
-1263.788720	32.603471	3.276506
-1261.731598	19.689396	3.286502
-1259.600706	22.809170	3.296499
-1257.733312	26.140054	3.306496
-1256.001566	16.028385	3.316493
-1254.256968	27.850927	3.326490
-1252.412626	23.645010	3.336486
-1250.348701	22.612135	3.346483
-1248.525149	17.140171	3.356480
-1246.667864	23.871902	3.366477
-1244.482900	33.071011	3.376474
-1242.934575	24.922769	3.386470
-1241.264511	19.750089	3.396467
-1239.183519	16.260991	3.406464
-1237.327357	22.475053	3.416461
-1235.332838	24.760950	3.426458
-1233.647318	17.013887	3.436454
-1231.495109	28.728590	3.446451
-1229.515308	23.032698	3.456448
-1228.055772	26.777800	3.466445
-1226.075535	37.542740	3.476442
-1224.031500	24.716040	3.486438
-1222.141148	24.503541	3.496435
-1220.445385	30.718030	3.506432
-1218.395902	23.163763	3.516429
-1216.574509	26.544671	3.526426
-1215.111401	29.978181	3.536422
-1213.053051	32.249148	3.546419
-1210.888454	18.435346	3.556416
-1209.336146	34.100002	3.566413
-1206.868624	21.515000	3.576410
-1205.313321	32.717403	3.586406
-1203.575175	23.755707	3.596403
-1201.681899	22.020763	3.606400
-1199.751280	23.396458	3.616397
-1197.911041	33.939107	3.626394
-1195.818258	28.296208	3.636390
-1193.992599	33.020040	3.646387
-1192.251239	19.428704	3.656384
-1190.663372	31.483212	3.666381
-1188.630947	22.520222	3.676378
-1186.613456	26.494994	3.686374
-1184.621500	26.599400	3.696371
-1182.691791	21.235223	3.706368
-1180.888234	23.215433	3.716365
-1179.219444	21.238553	3.726362
-1177.295519	13.807039	3.736358
-1175.209903	13.462288	3.746355
-1173.377495	16.944091	3.756352
-1171.533831	24.110668	3.766349
-1169.659794	25.479654	3.776346
-1168.099490	26.163105	3.786342
-1165.994657	15.200802	3.796339
-1164.001550	20.150475	3.806336
-1161.938186	14.894394	3.816333
-1160.329193	32.060961	3.826330
-1158.661985	20.723451	3.836326
-1156.405583	27.547708	3.846323
-1154.732294	24.123915	3.856320
-1152.829172	24.430443	3.866317
-1151.084247	20.920986	3.876314
-1148.999755	26.599683	3.886310
-1146.872984	25.509479	3.896307
-1145.221777	26.508378	3.906304
-1143.524313	24.436941	3.916301
-1141.604292	24.974442	3.926298
-1139.704779	20.093516	3.936294
-1137.957784	28.341302	3.946291
-1135.892122	20.258763	3.956288
-1133.964557	19.287278	3.966285
-1132.205626	24.189192	3.976282
-1130.300426	26.742085	3.986278
-1128.376814	29.456234	3.996275
-1126.608176	30.731600	4.006272
-1124.708441	24.642840	4.016269
-1122.776640	28.479812	4.026266
-1120.985086	21.952082	4.036262
-1118.789035	18.937274	4.046259
-1117.374833	20.263036	4.056256
-1115.756943	30.921851	4.066253
-1113.401040	25.819516	4.076250
-1111.140970	34.424161	4.086246
-1109.829739	25.009809	4.096243
-1107.516651	26.475962	4.106240
-1105.787877	26.472551	4.116237
-1104.135305	27.449157	4.126234
-1102.215981	19.001664	4.136230
-1100.181279	28.267588	4.146227
-1098.113130	29.547162	4.156224
-1096.598031	23.333655	4.166221
-1094.867810	33.551391	4.176218
-1092.748354	31.545103	4.186214
-1090.721896	23.078898	4.196211
-1088.979203	26.707747	4.206208
-1087.332468	33.212798	4.216205
-1085.518601	20.454601	4.226202
-1083.431858	18.298830	4.236198
-1081.407050	30.839279	4.246195
-1079.491051	26.738860	4.256192
-1077.787852	24.647607	4.266189
-1075.941529	23.847049	4.276186
-1074.084268	26.012951	4.286182
-1071.871917	17.832793	4.296179
-1070.262258	26.022084	4.306176
-1068.502777	22.927169	4.316173
-1066.305236	32.460743	4.326170
-1064.831869	31.568286	4.336166
-1062.969382	22.411541	4.346163
-1060.609588	22.673513	4.356160
-1058.983406	25.547395	4.366157
-1057.151242	29.561404	4.376154
-1055.204959	28.890125	4.386150
-1053.287673	19.794092	4.396147
-1051.529248	25.973429	4.406144
-1049.562246	29.386443	4.416141
-1047.732760	19.387155	4.426138
-1045.764851	22.735294	4.436134
-1043.965783	23.560625	4.446131
-1041.956884	24.616059	4.456128
-1040.285256	26.038052	4.466125
-1038.492834	24.865646	4.476122
-1036.220889	21.199346	4.486118
-1034.549589	20.797842	4.496115
-1032.909385	26.100905	4.506112
-1030.947275	30.057838	4.516109
-1028.751100	23.163894	4.526106
-1027.138705	20.739857	4.536102
-1025.440407	28.376625	4.546099
-1023.170690	23.570774	4.556096
-1021.422406	31.131662	4.566093
-1019.777852	24.011766	4.576090
-1017.935935	22.654630	4.586086
-1015.705281	21.164272	4.596083
-1014.021171	23.713154	4.606080
-1012.180824	24.863463	4.616077
-1010.362077	25.867239	4.626074
-1008.068084	24.925665	4.636070
-1006.253704	24.101852	4.646067
-1004.548205	17.600598	4.656064
-1002.661472	18.176694	4.666061
-1000.996951	20.191914	4.676058
-998.957438	23.460753	4.686054
-996.744614	25.113567	4.696051
-995.360295	17.729017	4.706048
-993.214767	29.992896	4.716045
-991.684167	18.069482	4.726042
-989.431305	23.877708	4.736038
-987.750711	22.535344	4.746035
-986.091145	16.507206	4.756032
-983.803448	17.244963	4.766029
-982.178370	15.993582	4.776026
-980.338244	15.751419	4.786022
-978.055910	11.360407	4.796019
-976.404624	30.266562	4.806016
-974.361804	23.035637	4.816013
-972.627741	36.108979	4.826010
-970.965182	34.385853	4.836006
-969.046470	26.303261	4.846003
-966.984451	24.312586	4.856000
-965.047321	27.441524	4.865997
-963.194703	31.826525	4.875994
-961.814495	28.792339	4.885990
-959.475715	19.884739	4.895987
-957.667360	24.379444	4.905984
-955.704705	28.083742	4.915981
-954.042213	34.120621	4.925978
-951.926333	26.518054	4.935974
-950.115577	22.661919	4.945971
-948.300396	21.896439	4.955968
-946.272281	27.882747	4.965965
-944.672133	22.448303	4.975962
-943.030842	24.236772	4.985958
-940.549853	24.837882	4.995955
-938.545206	25.096774	5.005952
-937.117408	25.998925	5.015949
-935.390580	30.081981	5.025946
-933.354250	22.717926	5.035942
-931.260701	26.300268	5.045939
-929.400693	27.565913	5.055936
-927.759878	29.158693	5.065933
-925.647666	29.005688	5.075930
-923.878104	28.359618	5.085926
-921.951117	22.247707	5.095923
-919.929394	25.145278	5.105920
-918.196328	27.455894	5.115917
-916.519416	23.381203	5.125914
-914.787246	27.120812	5.135910
-912.560067	27.579391	5.145907
-910.974295	26.277504	5.155904
-908.788166	29.249843	5.165901
-907.109309	30.958127	5.175898
-904.782547	28.380474	5.185894
-903.363853	32.678603	5.195891
-901.424735	20.865165	5.205888
-899.398867	35.066567	5.215885
-897.636713	29.123123	5.225882
-895.908563	23.485097	5.235878
-893.760009	33.756109	5.245875
-891.776832	33.510089	5.255872
-890.169863	30.997015	5.265869
-888.335449	28.032343	5.275866
-886.291731	28.933935	5.285862
-884.759149	26.961670	5.295859
-882.648506	15.637104	5.305856
-880.743978	21.324305	5.315853
-878.852010	24.117931	5.325850
-876.945607	19.730278	5.335846
-874.964588	19.494090	5.345843
-873.077517	17.635671	5.355840
-871.356041	21.400705	5.365837
-869.645479	22.210324	5.375834
-867.638742	16.136228	5.385830
-865.887147	14.657871	5.395827
-863.741700	23.093216	5.405824
-861.861286	15.708361	5.415821
-860.258846	32.841508	5.425818
-858.315696	26.910204	5.435814
-856.270649	20.433702	5.445811
-854.325381	27.254336	5.455808
-852.755607	28.111737	5.465805
-850.915523	25.929291	5.475802
-848.724943	23.742912	5.485798
-846.730923	16.690408	5.495795
-845.205455	16.459184	5.505792
-843.296434	24.746046	5.515789
-841.210034	29.231132	5.525786
-839.397252	23.500673	5.535782
-837.465705	19.765827	5.545779
-835.732670	22.629104	5.555776
-834.019957	24.576748	5.565773
-831.988833	23.922088	5.575770
-829.862159	17.727802	5.585766
-828.115031	17.709032	5.595763
-826.351760	18.908124	5.605760
-824.622267	20.044726	5.615757
-822.387540	22.477310	5.625754
-820.634601	21.137708	5.635750
-818.972985	20.231098	5.645747
-816.955883	17.990382	5.655744
-814.971396	16.373786	5.665741
-813.307666	18.480843	5.675738
-811.269189	15.739381	5.685734
-809.387339	25.680503	5.695731
-807.708175	21.610261	5.705728
-805.648393	24.580792	5.715725
-803.847662	23.230404	5.725722
-802.070017	31.252538	5.735718
-800.137134	23.917754	5.745715
-798.051478	23.287562	5.755712
-796.188425	26.592686	5.765709
-794.685501	24.809942	5.775706
-792.352317	22.981321	5.785702
-790.468728	23.387577	5.795699
-788.836942	18.207104	5.805696
-786.886147	20.677213	5.815693
-785.084264	21.650706	5.825690
-783.258155	27.483152	5.835686
-781.558021	33.694135	5.845683
-779.547824	22.058880	5.855680
-777.503921	25.358795	5.865677
-775.479301	29.831714	5.875674
-773.588972	24.073118	5.885670
-771.689433	22.724328	5.895667
-770.132106	28.122938	5.905664
-768.379472	24.681987	5.915661
-766.388780	27.036798	5.925658
-764.287934	23.781756	5.935654
-762.421890	28.197933	5.945651
-760.536972	24.825838	5.955648
-758.553657	20.222312	5.965645
-756.913209	30.637828	5.975642
-755.159973	27.784118	5.985638
-753.354612	24.173709	5.995635
-751.308094	22.932487	6.005632
-749.432882	28.409769	6.015629
-747.342360	26.563137	6.025626
-745.483098	34.305452	6.035622
-743.898417	28.069973	6.045619
-741.995417	31.929247	6.055616
-739.780354	32.167311	6.065613
-738.103629	29.527932	6.075610
-736.211632	24.531677	6.085606
-734.587544	27.188249	6.095603
-732.501040	30.579285	6.105600
-730.703977	29.036920	6.115597
-728.870200	26.888729	6.125594
-727.013129	15.146946	6.135590
-724.967501	20.788050	6.145587
-723.010643	25.344472	6.155584
-721.123128	22.592476	6.165581
-719.436691	25.164889	6.175578
-717.419040	26.947052	6.185574
-715.495106	22.908801	6.195571
-713.777652	25.037344	6.205568
-711.967093	36.442488	6.215565
-709.910885	28.867021	6.225562
-708.006206	27.291686	6.235558
-706.437334	34.720467	6.245555
-704.287569	27.292674	6.255552
-702.463044	20.188423	6.265549
-700.857510	29.614895	6.275546
-698.613673	32.568743	6.285542
-696.672493	26.055284	6.295539
-694.959130	26.212523	6.305536
-693.084042	19.701737	6.315533
-691.080477	33.684298	6.325530
-689.584359	33.105783	6.335526
-687.573345	22.441451	6.345523
-685.461563	30.268191	6.355520
-683.636648	24.205925	6.365517
-682.066363	28.731008	6.375514
-679.756029	19.444545	6.385510
-678.183916	29.829995	6.395507
-676.201979	23.155313	6.405504
-674.608479	29.318686	6.415501
-672.463997	33.156799	6.425498
-670.674152	26.725959	6.435494
-668.778577	25.167898	6.445491
-666.888186	26.618359	6.455488
-664.844979	26.399250	6.465485
-662.795465	31.345105	6.475482
-661.157004	25.877873	6.485478
-659.239769	24.725278	6.495475
-657.447310	26.841879	6.505472
-655.789731	29.190019	6.515469
-653.608987	33.586002	6.525466
-651.895692	29.838807	6.535462
-649.898299	26.043061	6.545459
-648.057254	21.991266	6.555456
-646.380990	34.117352	6.565453
-644.330515	31.945651	6.575450
-642.379046	33.108497	6.585446
-640.499331	30.544112	6.595443
-638.567120	36.520772	6.605440
-636.795508	33.983135	6.615437
-635.009277	31.343696	6.625434
-633.105649	33.065210	6.635430
-631.089222	32.672001	6.645427
-629.387753	25.292216	6.655424
-627.452426	29.249047	6.665421
-625.435533	25.838600	6.675418
-623.647616	28.224355	6.685414
-621.922029	32.145234	6.695411
-619.784437	30.654325	6.705408
-617.894794	30.674514	6.715405
-616.222913	34.149272	6.725402
-614.102384	28.080871	6.735398
-612.565246	27.877931	6.745395
-610.551435	25.825793	6.755392
-608.699342	27.912379	6.765389
-606.752388	33.076764	6.775386
-604.829690	34.676841	6.785382
-603.161186	27.627581	6.795379
-601.148384	27.331285	6.805376
-599.273101	31.182478	6.815373
-597.499729	28.031998	6.825370
-595.567706	26.723943	6.835366
-593.681864	25.709039	6.845363
-591.823161	41.393161	6.855360
-590.064781	30.535586	6.865357
-588.119820	30.589591	6.875354
-585.956547	28.968301	6.885350
-584.123264	34.409797	6.895347
-582.310777	31.030461	6.905344
-580.660502	36.145958	6.915341
-578.442497	33.751770	6.925338
-576.780400	27.148785	6.935334
-575.019640	32.570296	6.945331
-572.971584	27.244513	6.955328
-571.320723	34.102965	6.965325
-569.391598	31.669678	6.975322
-567.357811	24.855751	6.985318
-565.520601	24.753315	6.995315
-563.679432	24.809711	7.005312
-561.724866	26.827862	7.015309
-559.827967	25.725961	7.025306
-558.078652	29.268911	7.035302
-556.109826	29.387020	7.045299
-554.401423	33.817504	7.055296
-552.315813	32.049188	7.065293
-550.462889	24.372120	7.075290
-548.352389	24.143940	7.085286
-546.676198	28.593785	7.095283
-544.914310	23.149539	7.105280
-543.001210	18.682127	7.115277
-541.370776	22.817199	7.125274
-539.106309	18.366290	7.135270
-537.357046	18.748419	7.145267
-535.509711	19.867992	7.155264
-533.457522	25.149829	7.165261
-532.073224	21.810511	7.175258
-529.906186	29.388592	7.185254
-527.812978	25.280816	7.195251
-526.034800	24.921015	7.205248
-524.188418	25.286062	7.215245
-522.274763	18.000343	7.225242
-520.735511	19.945929	7.235238
-518.609664	24.136086	7.245235
-516.749734	27.391417	7.255232
-514.911127	25.053153	7.265229
-513.033380	20.978228	7.275226
-511.018194	25.347110	7.285222
-509.216928	23.407948	7.295219
-507.165322	25.319072	7.305216
-505.398796	30.809187	7.315213
-503.719294	34.770674	7.325210
-501.540771	29.351481	7.335206
-499.929062	25.939542	7.345203
-497.951097	25.811518	7.355200
-496.038274	21.606274	7.365197
-494.112906	30.263450	7.375194
-492.266490	22.707454	7.385190
-490.436003	28.310514	7.395187
-488.742811	26.518094	7.405184
-487.007142	31.403718	7.415181
-484.776555	24.656311	7.425178
-482.791961	17.289821	7.435174
-480.769380	27.093509	7.445171
-479.144267	30.703723	7.455168
-477.340328	24.169719	7.465165
-475.572770	23.825862	7.475162
-473.769823	39.686358	7.485158
-471.694392	30.848086	7.495155
-469.889930	23.682466	7.505152
-467.772018	32.608895	7.515149
-465.764221	24.768212	7.525146
-464.043994	29.037413	7.535142
-462.539626	31.026504	7.545139
-460.875549	31.051266	7.555136
-458.778062	24.621962	7.565133
-456.391214	18.187499	7.575130
-454.626225	28.296019	7.585126
-452.889229	28.201780	7.595123
-451.012790	32.386048	7.605120
-449.152333	27.764491	7.615117
-447.510020	36.536387	7.625114
-445.252133	28.654198	7.635110
-443.540762	24.716412	7.645107
-441.463410	24.732027	7.655104
-439.811802	33.042998	7.665101
-437.981628	31.686601	7.675098
-436.053333	27.439458	7.685094
-434.282783	28.325074	7.695091
-432.385103	26.458987	7.705088
-430.292426	23.125011	7.715085
-428.593419	28.423877	7.725082
-426.557132	27.337713	7.735078
-424.580437	28.405139	7.745075
-423.180891	29.468423	7.755072
-421.117629	32.959767	7.765069
-419.067501	41.702877	7.775066
-417.191616	31.554492	7.785062
-415.196573	27.089878	7.795059
-413.472394	23.952121	7.805056
-411.917709	28.999328	7.815053
-409.621792	28.141700	7.825050
-407.995408	32.421194	7.835046
-406.156543	24.710157	7.845043
-404.095072	27.655520	7.855040
-402.395011	29.434991	7.865037
-400.330535	31.595192	7.875034
-398.575529	24.928537	7.885030
-396.803317	22.856738	7.895027
-394.617509	31.204012	7.905024
-393.156112	27.255653	7.915021
-390.878459	26.402539	7.925018
-388.911274	28.011479	7.935014
-387.156961	26.305678	7.945011
-385.323787	25.218825	7.955008
-383.486905	27.129611	7.965005
-381.784473	35.533560	7.975002
-379.854342	24.882364	7.984998
-377.838791	28.206111	7.994995
-376.011745	25.577711	8.004992
-374.298590	24.011115	8.014989
-372.061729	19.304253	8.024986
-370.216212	29.249997	8.034982
-368.285805	23.344781	8.044979
-366.622390	27.452612	8.054976
-364.897285	28.801823	8.064973
-363.108362	24.169647	8.074970
-360.888685	37.216515	8.084966
-358.860569	25.629219	8.094963
-357.045453	29.231288	8.104960
-355.648758	24.701214	8.114957
-353.889461	27.162797	8.124954
-351.769614	31.169345	8.134950
-349.422770	25.859189	8.144947
-347.680927	23.031269	8.154944
-346.141297	28.813511	8.164941
-344.387117	28.195588	8.174938
-342.043739	22.213404	8.184934
-340.276824	20.767714	8.194931
-338.310807	24.096246	8.204928
-336.602935	36.198602	8.214925
-334.765983	31.705609	8.224922
-332.761810	34.955430	8.234918
-330.833075	27.533233	8.244915
-329.047153	36.744896	8.254912
-327.395664	25.374060	8.264909
-325.695211	34.228341	8.274906
-323.378983	30.672459	8.284902
-321.390283	29.443989	8.294899
-319.521493	29.748780	8.304896
-317.729460	32.393048	8.314893
-316.083334	31.817657	8.324890
-314.238863	31.085874	8.334886
-312.363683	29.221891	8.344883
-310.206664	28.206544	8.354880
-308.277774	27.189726	8.364877
-306.563062	25.856598	8.374874
-304.659804	22.076156	8.384870
-302.935044	32.563838	8.394867
-300.941311	26.637508	8.404864
-299.423019	33.724162	8.414861
-297.241629	42.700629	8.424858
-294.771490	34.765736	8.434854
-293.349845	30.236446	8.444851
-291.816236	39.998391	8.454848
-289.825618	35.375114	8.464845
-287.836577	28.284353	8.474842
-285.986937	33.819794	8.484838
-283.844111	26.777113	8.494835
-282.105811	31.886675	8.504832
-280.330729	29.122964	8.514829
-278.509113	29.462157	8.524826
-276.202325	30.458068	8.534822
-274.695622	24.892119	8.544819
-273.276601	34.482903	8.554816
-271.110567	29.383248	8.564813
-268.959321	28.351491	8.574810
-267.173313	30.153655	8.584807
-264.944591	27.107555	8.594803
-263.291605	29.423556	8.604800
-261.869384	33.131047	8.614797
-260.148668	39.579142	8.624794
-257.866066	37.249137	8.634791
-255.504274	32.729262	8.644787
-253.954347	34.395446	8.654784
-252.236529	34.358095	8.664781
-250.298059	25.044521	8.674778
-248.270934	28.628624	8.684775
-246.871044	38.213010	8.694771
-244.660348	28.666523	8.704768
-242.775050	37.535576	8.714765
-240.817149	29.660395	8.724762
-239.126885	29.932169	8.734759
-237.185081	24.451519	8.744755
-235.148098	24.450073	8.754752
-233.543765	25.010286	8.764749
-231.402876	27.125283	8.774746
-229.504202	24.608707	8.784743
-227.797769	22.686466	8.794739
-225.910596	24.182005	8.804736
-224.037736	25.326168	8.814733
-222.144187	28.284286	8.824730
-220.356578	22.509333	8.834727
-218.613487	22.886366	8.844723
-216.479733	23.919425	8.854720
-214.372123	32.719862	8.864717
-212.576954	26.695826	8.874714
-211.139323	28.758885	8.884711
-209.185096	29.627985	8.894707
-207.112724	28.203107	8.904704
-205.240434	35.530153	8.914701
-203.299295	33.054184	8.924698
-201.509627	40.503364	8.934695
-199.630127	34.576394	8.944691
-197.684246	38.539804	8.954688
-196.062693	35.799076	8.964685
-193.761351	27.648078	8.974682
-191.609542	27.713600	8.984679
-190.062701	21.721320	8.994675
-188.444396	22.819300	9.004672
-186.744640	28.152967	9.014669
-184.659184	27.082840	9.024666
-182.567074	31.933920	9.034663
-180.657669	26.515321	9.044659
-179.024146	24.369500	9.054656
-177.534807	33.325483	9.064653
-175.145068	30.408493	9.074650
-173.167208	29.428174	9.084647
-171.547037	26.791888	9.094643
-169.682528	24.599737	9.104640
-167.594320	34.503776	9.114637
-166.081313	34.799153	9.124634
-164.073312	28.861177	9.134631
-162.031379	30.467851	9.144627
-160.236430	29.554625	9.154624
-158.452720	32.208239	9.164621
-156.482842	27.752579	9.174618
-154.479587	28.002884	9.184615
-153.214939	29.253636	9.194611
-150.772772	32.269518	9.204608
-148.738935	35.413719	9.214605
-147.187730	34.629393	9.224602
-145.194289	32.782979	9.234599
-143.130101	23.215750	9.244595
-141.501983	29.973954	9.254592
-139.705226	24.298642	9.264589
-138.033449	31.259870	9.274586
-135.868378	24.910034	9.284583
-133.810451	32.417504	9.294579
-132.093439	28.652699	9.304576
-130.598521	26.293779	9.314573
-128.433175	23.398432	9.324570
-126.190599	18.940333	9.334567
-124.643349	34.377767	9.344563
-122.631322	31.903180	9.354560
-120.810267	24.182548	9.364557
-119.097301	21.897782	9.374554
-117.083873	28.479266	9.384551
-114.848898	30.923547	9.394547
-113.290451	28.374510	9.404544
-111.826912	21.093014	9.414541
-109.641206	24.656671	9.424538
-107.671880	29.525833	9.434535
-105.915135	29.929189	9.444531
-103.734950	22.362832	9.454528
-102.229725	29.439078	9.464525
-100.265839	27.987393	9.474522
-98.156567	26.092537	9.484519
-96.419888	25.168130	9.494515
-94.583009	25.953422	9.504512
-92.617776	30.002247	9.514509
-90.956233	31.287594	9.524506
-88.872429	41.192417	9.534503
-86.617604	25.348869	9.544499
-85.421531	29.577261	9.554496
-83.675760	31.100212	9.564493
-81.640506	32.463300	9.574490
-79.474018	27.845284	9.584487
-77.496839	28.878188	9.594483
-75.741201	31.577394	9.604480
-73.942999	31.228942	9.614477
-71.913811	28.503778	9.624474
-70.133333	34.211476	9.634471
-68.458890	23.756015	9.644467
-66.241999	35.215316	9.654464
-64.612397	28.909918	9.664461
-62.647566	35.483419	9.674458
-60.664617	25.705014	9.684455
-58.560250	28.530163	9.694451
-57.334746	31.547632	9.704448
-55.679111	32.641327	9.714445
-53.271342	26.683865	9.724442
-51.282083	34.584451	9.734439
-49.451408	24.852451	9.744435
-47.827532	29.996238	9.754432
-45.905510	30.570627	9.764429
-43.831529	33.116445	9.774426
-41.827121	31.795701	9.784423
-40.311111	28.533523	9.794419
-38.181488	26.760201	9.804416
-36.333474	25.432835	9.814413
-34.646174	29.322377	9.824410
-32.650652	29.394028	9.834407
-30.577976	29.323906	9.844403
-29.255322	26.826747	9.854400
-27.173253	32.263748	9.864397
-25.168484	33.241770	9.874394
-23.345181	31.548904	9.884391
-21.267810	27.046201	9.894387
-19.157416	31.532957	9.904384
-17.413974	24.416845	9.914381
-15.805586	27.831123	9.924378
-14.097367	32.374147	9.934375
-12.253525	32.970508	9.944371
-10.023286	30.576458	9.954368
-8.066903	27.855066	9.964365
-6.377603	23.125351	9.974362
-4.710761	34.025130	9.984359
-3.271595	58.143104	9.994355
-2.378244	90.892976	10.004352
-1.293324	160.260994	10.014349
0.000000	213.792049	10.019354
0.434502	258.787744	10.024359
1.094007	300.370045	10.029363
1.157426	345.527702	10.034368
1.846642	374.009586	10.039373
2.623343	395.126181	10.044378
2.976832	425.426244	10.049383
3.205648	439.669966	10.054387
3.291454	454.590920	10.059392
3.821952	456.021691	10.064397
3.420476	472.873228	10.069402
3.424070	473.675300	10.074407
3.839491	472.735452	10.079411
3.750910	501.511963	10.084416
3.833851	506.048061	10.089421
4.087450	513.425294	10.094426
4.179411	509.205079	10.099431
4.444979	514.404301	10.104435
4.216822	528.834541	10.109440
4.354933	513.600284	10.114445
4.129034	520.929435	10.119450
4.111688	536.275341	10.124455
4.290416	523.319508	10.129459
4.426910	530.171404	10.134464
4.199189	530.442697	10.139469
4.418785	529.202936	10.144474
4.379677	528.430203	10.149479
4.515851	535.767835	10.154483
4.505165	556.978731	10.159488
5.021819	565.892499	10.164493
4.917559	569.332577	10.169498
4.844541	563.481348	10.174503
4.964382	572.247115	10.179507
4.887093	586.369506	10.184512
4.984535	582.435390	10.189517
5.012246	585.969533	10.194522
5.316186	588.261174	10.199527
5.150034	583.609042	10.204531
4.791192	589.858762	10.209536
4.868746	592.740006	10.214541
5.122198	592.980275	10.219546
5.128716	600.396967	10.224551
5.398138	600.986337	10.229555
5.045560	605.107831	10.234560
5.531203	597.191621	10.239565
5.370893	598.415646	10.244570
5.392335	615.130503	10.249575
5.733947	593.481994	10.254579
5.496605	604.644870	10.259584
5.358758	604.971211	10.264589
5.668423	608.408346	10.269594
5.502975	622.325646	10.274599
5.700889	610.986149	10.279603
5.480841	610.672767	10.284608
5.843495	612.373171	10.289613
5.717015	616.340335	10.294618
5.784893	636.337219	10.299623
6.041525	635.443190	10.304627
5.992794	645.568372	10.309632
6.078182	651.308878	10.314637
6.241727	642.950453	10.319642
5.869331	645.185991	10.324647
6.332764	646.379907	10.329651
6.386092	655.284063	10.334656
6.693006	650.619524	10.339661
6.403969	648.055869	10.344666
6.656439	647.334386	10.349671
6.242378	634.148171	10.354675
5.946936	644.971850	10.359680
6.493963	659.423642	10.364685
6.662770	657.821400	10.369690
6.141967	661.540826	10.374695
6.385898	657.800935	10.379699
6.391469	658.061824	10.384704
6.515120	652.466184	10.389709
6.473378	661.820734	10.394714
6.458613	660.982612	10.399719
6.580952	667.193454	10.404723
6.660464	690.429095	10.409728
6.913322	685.437287	10.414733
6.860737	691.583006	10.419738
6.661060	694.767105	10.424743
6.974908	694.325981	10.429747
6.937982	706.201265	10.434752
6.821188	707.763700	10.439757
6.942322	713.347145	10.444762
6.788552	703.432432	10.449767
7.563874	710.731276	10.454771
7.259651	728.718739	10.459776
7.272924	734.492858	10.464781
7.629366	744.384748	10.469786
7.534766	741.775868	10.474791
7.739809	729.457456	10.479795
7.275012	731.770823	10.484800
7.622109	732.502346	10.489805
7.518526	745.958899	10.494810
7.114298	754.690105	10.499815
7.713763	733.881750	10.504819
7.639139	746.417499	10.509824
7.543069	743.580201	10.514829
7.497387	746.630941	10.519834
7.531399	751.665340	10.524839
7.757232	750.803026	10.529843
7.572861	762.705030	10.534848
7.692128	769.890940	10.539853
7.717870	791.137368	10.544858
7.615411	780.798111	10.549863
7.832000	779.215041	10.554867
7.926359	792.230065	10.559872
8.093475	798.102669	10.564877
8.315861	802.465232	10.569882
8.140704	823.724831	10.574887
8.406470	818.817649	10.579891
7.918026	833.636634	10.584896
8.203594	830.637518	10.589901
8.356445	833.577761	10.594906
8.170112	839.859993	10.599911
8.302608	835.593794	10.604915
8.171660	827.916162	10.609920
8.458746	855.756683	10.614925
8.518629	855.958450	10.619930
8.972685	865.237198	10.624935
8.876847	871.867701	10.629939
8.928372	872.460303	10.634944
9.109126	869.944669	10.639949
9.114672	865.334443	10.644954
8.867361	878.090236	10.649959
9.159951	852.181999	10.654963
9.146996	873.147720	10.659968
8.948474	867.212310	10.664973
9.197369	868.233891	10.669978
9.257301	880.634754	10.674983
9.520137	869.125430	10.679987
9.238684	885.743837	10.684992
9.177673	873.970782	10.689997
9.512889	874.302093	10.695002
8.838489	883.667818	10.700007
9.339965	882.468219	10.705011
9.468757	878.905908	10.710016
9.368582	879.831786	10.715021
9.654361	882.654643	10.720026
9.631639	891.418113	10.725031
9.794465	878.019806	10.730035
9.440906	879.927527	10.735040
9.578437	882.762993	10.740045
9.671380	883.196026	10.745050
9.409378	899.800308	10.750055
9.852119	910.271472	10.755059
9.821760	913.423880	10.760064
9.913999	914.924608	10.765069
10.164771	914.331116	10.770074
9.875844	918.951892	10.775079
10.098449	918.079045	10.780083
9.968481	935.915967	10.785088
10.090534	925.383101	10.790093
10.424651	920.018710	10.795098
10.148224	924.110799	10.800103
10.230041	918.081766	10.805107
10.448090	921.658169	10.810112
10.424854	926.290182	10.815117
10.173873	922.510899	10.820122
10.225532	940.085469	10.825127
10.534119	937.809627	10.830131
10.638638	956.298291	10.835136
10.745019	957.236956	10.840141
10.847307	968.060510	10.845146
10.831295	966.656448	10.850151
10.624066	960.408579	10.855155
10.752737	969.305641	10.860160
10.857389	967.956447	10.865165
10.729309	966.975535	10.870170
10.751380	968.011227	10.875175
11.267953	957.450099	10.880179
11.047201	965.552927	10.885184
10.995573	964.108816	10.890189
11.328820	963.748168	10.895194
10.869746	970.871891	10.900199
11.109269	965.233994	10.905203
11.241283	971.520694	10.910208
10.924175	967.288328	10.915213
11.067552	975.995392	10.920218
10.653076	984.280519	10.925223
11.416157	977.024742	10.930227
11.272892	995.368478	10.935232
11.365713	995.989191	10.940237
11.786602	1000.305958	10.945242
11.341783	995.647681	10.950247
11.426688	1005.806990	10.955251
11.584171	1000.507016	10.960256
11.659889	993.901764	10.965261
11.626082	992.459538	10.970266
11.476003	1003.944688	10.975271
11.809196	1001.212330	10.980275
11.949595	1005.843497	10.985280
11.775958	1022.337631	10.990285
12.177331	1025.541043	10.995290
12.353085	1037.972451	11.000295
12.355937	1025.170380	11.005299
12.208124	1011.129224	11.010304
12.041856	998.046650	11.015309
12.367528	1004.258319	11.020314
11.887020	1005.803110	11.025319
12.230312	1024.592816	11.030323
12.047374	1028.178015	11.035328
12.037032	1039.047972	11.040333
12.621612	1039.599706	11.045338
12.146393	1035.584928	11.050343
12.280344	1041.393536	11.055347
12.699390	1033.777873	11.060352
12.732176	1039.444922	11.065357
12.847952	1038.426684	11.070362
12.543985	1047.416459	11.075367
12.663268	1041.083356	11.080371
12.529362	1046.472647	11.085376
12.743047	1039.482670	11.090381
12.786583	1043.591563	11.095386
12.898570	1050.767735	11.100391
13.125872	1057.513934	11.105395
13.002631	1066.381853	11.110400
13.159222	1071.029382	11.115405
13.273638	1068.388679	11.120410
12.892176	1074.509749	11.125415
13.306535	1067.863062	11.130419
13.399837	1072.665766	11.135424
13.058915	1068.911830	11.140429
13.362258	1079.501547	11.145434
13.531577	1077.139089	11.150439
13.711270	1068.875615	11.155443
13.904843	1069.041868	11.160448
13.469252	1051.618292	11.165453
13.445839	1040.561346	11.170458
13.147099	1057.584828	11.175463
13.542954	1060.563625	11.180467
13.575505	1070.269286	11.185472
13.347874	1082.653113	11.190477
13.755320	1075.435093	11.195482
13.727992	1078.902443	11.200487
13.996647	1075.773513	11.205491
14.008434	1078.890848	11.210496
13.867009	1085.851995	11.215501
14.200079	1077.179275	11.220506
14.012778	1082.458825	11.225511
14.168052	1075.602727	11.230515
13.932763	1086.085980	11.235520
13.979808	1082.423119	11.240525
13.928345	1074.589174	11.245530
14.176034	1083.588746	11.250535
14.047852	1086.441405	11.255539
13.776700	1105.849622	11.260544
14.363046	1108.646657	11.265549
14.834626	1103.679742	11.270554
14.362244	1116.219333	11.275559
14.593204	1113.746112	11.280563
14.757580	1116.419647	11.285568
14.455276	1124.109794	11.290573
14.606346	1118.713029	11.295578
14.694167	1114.639956	11.300583
14.515405	1108.209286	11.305587
14.881427	1119.572779	11.310592
14.943083	1117.093448	11.315597
14.535318	1106.599230	11.320602
14.519990	1126.252095	11.325607
14.291706	1119.983861	11.330611
14.643412	1117.444070	11.335616
14.605288	1134.814001	11.340621
14.971734	1129.579996	11.345626
14.863424	1145.280102	11.350631
15.037454	1145.600861	11.355635
15.251479	1156.513966	11.360640
15.329446	1148.958957	11.365645
15.547623	1144.989661	11.370650
15.049450	1151.189304	11.375655
15.517184	1155.736768	11.380659
15.427456	1151.873355	11.385664
15.329959	1149.963455	11.390669
15.473570	1147.277079	11.395674
15.350825	1155.391188	11.400679
15.558546	1143.944056	11.405683
15.074866	1163.777335	11.410688
15.187906	1174.271321	11.415693
15.798318	1170.073872	11.420698
15.399290	1190.524468	11.425703
15.946937	1186.915771	11.430707
15.600513	1186.578378	11.435712
15.675370	1191.100210	11.440717
15.976033	1181.212031	11.445722
15.869376	1187.043307	11.450727
15.883247	1184.547932	11.455731
16.064334	1191.363067	11.460736
15.906204	1190.491011	11.465741
16.211307	1188.605197	11.470746
16.250933	1203.548482	11.475751
16.461676	1210.844600	11.480755
16.300521	1191.235564	11.485760
16.165891	1192.807203	11.490765
16.136844	1208.696586	11.495770
16.584518	1220.323103	11.500775
16.537063	1216.235309	11.505779
16.429890	1213.027526	11.510784
16.590245	1218.114475	11.515789
16.938559	1217.041785	11.520794
16.568582	1225.383028	11.525799
17.070680	1215.923167	11.530803
16.903253	1214.406038	11.535808
16.874128	1224.277759	11.540813
16.910225	1223.702728	11.545818
16.936682	1227.913746	11.550823
16.974364	1217.572323	11.555827
17.272359	1215.413247	11.560832
16.762988	1205.428754	11.565837
16.958326	1204.154961	11.570842
16.744456	1217.773047	11.575847
16.908675	1229.280781	11.580851
16.892294	1212.477699	11.585856
16.823911	1218.004837	11.590861
17.060119	1222.314861	11.595866
17.041376	1227.502922	11.600871
17.136843	1217.983341	11.605875
17.543973	1240.721326	11.610880
17.533717	1256.371218	11.615885
17.567315	1230.123570	11.620890
17.401040	1242.817871	11.625895
17.697820	1246.183099	11.630899
17.907012	1259.516120	11.635904
17.793462	1240.192740	11.640909
17.711083	1221.510970	11.645914
17.389544	1230.103111	11.650919
17.872291	1237.693326	11.655923
17.872417	1243.748868	11.660928
17.594496	1246.398360	11.665933
18.299732	1240.927347	11.670938
17.826582	1242.336944	11.675943
17.950899	1249.251049	11.680947
18.031844	1244.551403	11.685952
18.017010	1252.408654	11.690957
18.084931	1244.120331	11.695962
17.777965	1250.270593	11.700967
18.139471	1248.853595	11.705971
18.010378	1239.577979	11.710976
18.176190	1248.674294	11.715981
18.385442	1247.188542	11.720986
18.797608	1248.799125	11.725991
18.567782	1248.537749	11.730995
18.555745	1257.066345	11.736000
18.714257	1245.311588	11.741005
18.534690	1253.594089	11.746010
18.291039	1264.460430	11.751015
18.286270	1246.020140	11.756019
18.610573	1259.240181	11.761024
18.566096	1265.369080	11.766029
18.988078	1268.064631	11.771034
18.704570	1271.811012	11.776039
18.872414	1275.375011	11.781043
18.690660	1264.876166	11.786048
18.803855	1280.050649	11.791053
18.956462	1268.650057	11.796058
18.687624	1279.627660	11.801063
18.895850	1258.830502	11.806067
18.973073	1268.363588	11.811072
18.628106	1279.307602	11.816077
19.128651	1288.169197	11.821082
19.312792	1302.636942	11.826087
19.655764	1303.531584	11.831091
19.687858	1309.023806	11.836096
19.588630	1304.821241	11.841101
19.908717	1294.974042	11.846106
19.561506	1297.040076	11.851111
19.547124	1269.844364	11.856115
19.446739	1275.986916	11.861120
19.358438	1296.962115	11.866125
19.743442	1300.453634	11.871130
19.913266	1309.612426	11.876135
20.061467	1309.800113	11.881139
19.940420	1293.240716	11.886144
19.655761	1285.224655	11.891149
20.122188	1306.507203	11.896154
20.016486	1307.203751	11.901159
19.974179	1296.540712	11.906163
19.965257	1304.032767	11.911168
19.624216	1310.251568	11.916173
20.018615	1314.239915	11.921178
20.173702	1311.359289	11.926183
20.058663	1306.563150	11.931187
19.991988	1309.499083	11.936192
20.061313	1305.223900	11.941197
20.329714	1300.044898	11.946202
20.002790	1309.421700	11.951207
20.140355	1297.493622	11.956211
20.453081	1313.532032	11.961216
19.965458	1335.630709	11.966221
20.340645	1334.361334	11.971226
20.483902	1335.902855	11.976231
20.600093	1336.720131	11.981235
20.361128	1346.619099	11.986240
20.400742	1343.171827	11.991245
20.724124	1335.700579	11.996250
20.193629	1346.653736	12.001255
20.656512	1367.172104	12.006259
20.959218	1364.025066	12.011264
20.647335	1371.477171	12.016269
21.061110	1368.206757	12.021274
21.173304	1371.399605	12.026279
21.432240	1370.744869	12.031283
21.288000	1372.139861	12.036288
21.052789	1367.755538	12.041293
21.342551	1353.535440	12.046298
21.106509	1352.865039	12.051303
21.101615	1340.751488	12.056307
21.105184	1324.408725	12.061312
20.596820	1339.877959	12.066317
21.301381	1340.364838	12.071322
21.316222	1338.856470	12.076327
21.051334	1335.248032	12.081331
21.164200	1325.148433	12.086336
20.955185	1335.082040	12.091341
21.131320	1343.273160	12.096346
21.282437	1345.182442	12.101351
21.044064	1333.314300	12.106355
21.383229	1333.846847	12.111360
21.279990	1346.766153	12.116365
21.302551	1326.195635	12.121370
21.215287	1349.280738	12.126375
21.010042	1339.999858	12.131379
20.989258	1312.683660	12.136384
20.876149	1331.966042	12.141389
21.567339	1282.748846	12.146394
20.750405	1336.133570	12.151399
20.739708	1304.581596	12.156403
20.913874	1325.574896	12.161408
20.949745	1320.434554	12.166413
21.294557	1322.229357	12.171418
21.491098	1322.825655	12.176423
21.190379	1293.721699	12.181427
21.220271	1327.099902	12.186432
21.211402	1316.098773	12.191437
20.875713	1289.654452	12.196442
21.048261	1318.010881	12.201447
20.921514	1312.540085	12.206451
21.270474	1314.187566	12.211456
21.076013	1311.889405	12.216461
20.939506	1300.340937	12.221466
21.013073	1305.594727	12.226471
21.133653	1302.218129	12.231475
20.807453	1304.359662	12.236480
20.720792	1316.710164	12.241485
21.000947	1320.727775	12.246490
20.886568	1312.476377	12.251495
20.892556	1317.015543	12.256499
21.203332	1315.144577	12.261504
21.266176	1317.006433	12.266509
21.064902	1311.530179	12.271514
21.172547	1321.615119	12.276519
21.072324	1323.827844	12.281523
21.294873	1318.157825	12.286528
20.927704	1312.406830	12.291533
21.186365	1310.939998	12.296538
21.403226	1311.433705	12.301543
21.274526	1315.060785	12.306547
20.976244	1304.359722	12.311552
20.834222	1297.484708	12.316557
20.905167	1294.436155	12.321562
21.182784	1309.664867	12.326567
21.347237	1309.780575	12.331571
21.191243	1294.614488	12.336576
20.775254	1292.868913	12.341581
20.879644	1284.562134	12.346586
20.842289	1284.807803	12.351591
20.866411	1299.923974	12.356595
21.202154	1293.365421	12.361600
21.246144	1293.107677	12.366605
20.946801	1303.653343	12.371610
21.333637	1299.467867	12.376615
21.113591	1281.926051	12.381619
21.064521	1301.149291	12.386624
20.738518	1306.673400	12.391629
21.095724	1299.509017	12.396634
21.011177	1293.927416	12.401639
20.740073	1293.603237	12.406643
20.901601	1285.873977	12.411648
20.757086	1308.553403	12.416653
21.127839	1290.682370	12.421658
21.101393	1302.630588	12.426663
21.293529	1296.397719	12.431667
21.275414	1306.770794	12.436672
20.959320	1280.096280	12.441677
21.126144	1315.898498	12.446682
21.101584	1300.440201	12.451687
21.052503	1301.268067	12.456691
21.345003	1302.538195	12.461696
21.225011	1291.744046	12.466701
21.152439	1291.339313	12.471706
21.088782	1309.342738	12.476711
21.231292	1299.743060	12.481715
21.120214	1285.262109	12.486720
20.895612	1313.902655	12.491725
20.840367	1300.748481	12.496730
21.029431	1296.714401	12.501735
20.878708	1298.111998	12.506739
20.928991	1301.822491	12.511744
20.883169	1307.532146	12.516749
20.952618	1299.387053	12.521754
20.978746	1309.007164	12.526759
20.727764	1315.017634	12.531763
21.198654	1302.539636	12.536768
20.981595	1301.341078	12.541773
21.315156	1299.316667	12.546778
21.097504	1307.606851	12.551783
21.271863	1311.124088	12.556787
21.387458	1315.300412	12.561792
21.035256	1304.056009	12.566797
21.052309	1291.831763	12.571802
20.895976	1305.412368	12.576807
21.120143	1289.925446	12.581811
21.278420	1284.667820	12.586816
21.026217	1299.892723	12.591821
21.034682	1293.315410	12.596826
20.845263	1290.743632	12.601831
21.181484	1284.688060	12.606835
21.068398	1291.660554	12.611840
21.176528	1286.281615	12.616845
21.135508	1274.894556	12.621850
21.331228	1290.237238	12.626855
20.825802	1295.116595	12.631859
20.813883	1288.736503	12.636864
20.957980	1289.006847	12.641869
20.494264	1282.246232	12.646874
20.674533	1285.399817	12.651879
20.477876	1296.250800	12.656883
21.166633	1299.813718	12.661888
20.848508	1294.628925	12.666893
21.111935	1321.537397	12.671898
21.274773	1315.507891	12.676903
21.075631	1304.344731	12.681907
20.911045	1303.426388	12.686912
21.327912	1295.471888	12.691917
20.885150	1280.280595	12.696922
20.941902	1281.553631	12.701927
21.183330	1301.287206	12.706931
21.214147	1282.937388	12.711936
21.069234	1292.717237	12.716941
21.088622	1294.138161	12.721946
21.114837	1282.760873	12.726951
20.618369	1290.026334	12.731955
20.996163	1283.582504	12.736960
20.334756	1305.084374	12.741965
21.024596	1303.323259	12.746970
20.950047	1318.190256	12.751975
21.258354	1306.558215	12.756979
21.054112	1305.578389	12.761984
20.933054	1317.264164	12.766989
21.253256	1298.656852	12.771994
21.240781	1294.347411	12.776999
20.943530	1291.904798	12.782003
21.092646	1280.887957	12.787008
20.934092	1310.107747	12.792013
21.169938	1285.518254	12.797018
21.367806	1290.241273	12.802023
20.982020	1300.422252	12.807027
21.158742	1292.994920	12.812032
20.957376	1299.931037	12.817037
21.150464	1294.710433	12.822042
20.927191	1299.243584	12.827047
21.329193	1303.992394	12.832051
21.245874	1283.047737	12.837056
21.344163	1306.081096	12.842061
21.240082	1304.320461	12.847066
21.046411	1304.507485	12.852071
20.941130	1297.199251	12.857075
21.106824	1294.206548	12.862080
21.097905	1313.967456	12.867085
21.348599	1288.976615	12.872090
21.037745	1265.409503	12.877095
20.672170	1281.794197	12.882099
20.951944	1258.156541	12.887104
21.375657	1281.563735	12.892109
21.202358	1268.068871	12.897114
20.879174	1261.957639	12.902119
21.081635	1269.538962	12.907123
20.780211	1264.827761	12.912128
20.718131	1274.304223	12.917133
20.864871	1266.886417	12.922138
21.089698	1295.816366	12.927143
20.844101	1285.075374	12.932147
21.216679	1304.945730	12.937152
21.039153	1279.444461	12.942157
20.546598	1288.145917	12.947162
20.832360	1294.715744	12.952167
20.930005	1291.719703	12.957171
21.180252	1295.636421	12.962176
21.168461	1317.294890	12.967181
21.097366	1292.558800	12.972186
21.068617	1319.043934	12.977191
20.979985	1304.922088	12.982195
21.150663	1300.515621	12.987200
21.019144	1283.863287	12.992205
21.033695	1285.248712	12.997210
21.069454	1288.870054	13.002215
20.870392	1260.401239	13.007219
21.160195	1286.625766	13.012224
21.073189	1283.542484	13.017229
21.228962	1266.122092	13.022234
21.233986	1275.805473	13.027239
20.800704	1292.894846	13.032243
20.961708	1272.458442	13.037248
21.032490	1275.795070	13.042253
21.080091	1279.886035	13.047258
21.072649	1270.404913	13.052263
21.057622	1282.237752	13.057267
21.161216	1276.364371	13.062272
20.844969	1274.471999	13.067277
20.657142	1273.171009	13.072282
20.617859	1277.565994	13.077287
20.914544	1281.087366	13.082291
21.249577	1271.922203	13.087296
20.789410	1270.828658	13.092301
21.239457	1287.475924	13.097306
21.051313	1294.018840	13.102311
21.202637	1269.837098	13.107315
21.427464	1291.404169	13.112320
20.974355	1275.933830	13.117325
20.713931	1279.064666	13.122330
21.045552	1289.798263	13.127335
21.036343	1265.810871	13.132339
20.823878	1277.290418	13.137344
21.032586	1279.089579	13.142349
20.903835	1281.565471	13.147354
20.696394	1281.751537	13.152359
20.904919	1285.055158	13.157363
21.011303	1279.865736	13.162368
20.786231	1287.124176	13.167373
20.778208	1287.116005	13.172378
21.181922	1303.999342	13.177383
21.110164	1303.591325	13.182387
21.019451	1288.939963	13.187392
20.976440	1295.300455	13.192397
21.115596	1279.735640	13.197402
21.108988	1287.402361	13.202407
20.982154	1289.430089	13.207411
20.916086	1269.351612	13.212416
20.778144	1284.526733	13.217421
20.967900	1310.130165	13.222426
21.312278	1308.901976	13.227431
21.116271	1300.352941	13.232435
21.207671	1285.953235	13.237440
21.092234	1279.304227	13.242445
21.120107	1281.371932	13.247450
20.969823	1290.696892	13.252455
20.833468	1288.736400	13.257459
20.986894	1289.601351	13.262464
21.248118	1292.844527	13.267469
20.934468	1291.926308	13.272474
21.319990	1287.275838	13.277479
20.960220	1289.952586	13.282483
21.149972	1286.104483	13.287488
20.775891	1282.234352	13.292493
20.825437	1298.108142	13.297498
20.933154	1293.353747	13.302503
20.833088	1292.874551	13.307507
21.048567	1294.234235	13.312512
20.983401	1283.836629	13.317517
21.103189	1296.389152	13.322522
21.015658	1292.873862	13.327527
21.023392	1294.768160	13.332531
21.076489	1284.394268	13.337536
21.180072	1284.677382	13.342541
21.219005	1279.806228	13.347546
21.054383	1302.263345	13.352551
21.010239	1302.975305	13.357555
21.276927	1281.982705	13.362560
21.084949	1283.287531	13.367565
20.778962	1294.081835	13.372570
21.207784	1279.060604	13.377575
21.007237	1289.666195	13.382579
21.196438	1302.609779	13.387584
20.672732	1292.225383	13.392589
21.172929	1268.484742	13.397594
21.278578	1304.914862	13.402599
20.982838	1284.226440	13.407603
21.364076	1314.298435	13.412608
21.144772	1275.992502	13.417613
21.106423	1294.928592	13.422618
21.186031	1277.528221	13.427623
20.900080	1294.788062	13.432627
21.133041	1256.157725	13.437632
20.503878	1282.812683	13.442637
21.233301	1281.225031	13.447642
21.402606	1271.534364	13.452647
20.834355	1290.591243	13.457651
21.331181	1254.773140	13.462656
20.799822	1264.576764	13.467661
20.893900	1271.896254	13.472666
21.183785	1263.626132	13.477671
20.841175	1258.716496	13.482675
21.371307	1258.357554	13.487680
21.202631	1278.364672	13.492685
21.096682	1262.249185	13.497690
21.299581	1255.666107	13.502695
21.025332	1262.560214	13.507699
21.288077	1269.635177	13.512704
21.224411	1263.102499	13.517709
20.898757	1261.960690	13.522714
21.249074	1268.916027	13.527719
21.059456	1253.143483	13.532723
20.911517	1271.190267	13.537728
21.191625	1271.596612	13.542733
20.921843	1272.950118	13.547738
21.241649	1270.899520	13.552743
20.944752	1275.285134	13.557747
21.205919	1267.566799	13.562752
21.188582	1258.349039	13.567757
21.023412	1273.044363	13.572762
21.381794	1244.459853	13.577767
21.277088	1233.825737	13.582771
21.096388	1230.317438	13.587776
20.871932	1250.144180	13.592781
20.902658	1224.567210	13.597786
20.973547	1235.107388	13.602791
20.794655	1244.816931	13.607795
20.960459	1229.381961	13.612800
21.075262	1226.165575	13.617805
20.970723	1239.827744	13.622810
20.828046	1238.855449	13.627815
20.848330	1238.918457	13.632819
20.970855	1239.960223	13.637824
20.481996	1252.882608	13.642829
20.773701	1266.402749	13.647834
20.947933	1250.472822	13.652839
20.933505	1281.036795	13.657843
21.149651	1272.794199	13.662848
21.071152	1264.185440	13.667853
20.770559	1265.580131	13.672858
20.715369	1259.706853	13.677863
21.003625	1278.453629	13.682867
20.957422	1271.238488	13.687872
21.301364	1263.305099	13.692877
21.263487	1266.796254	13.697882
21.432133	1265.468366	13.702887
21.006529	1280.744562	13.707891
21.126515	1264.764924	13.712896
20.907302	1255.782796	13.717901
20.838494	1274.225397	13.722906
21.471164	1259.665261	13.727911
20.557422	1255.972682	13.732915
21.043179	1261.474525	13.737920
20.670837	1269.699474	13.742925
20.710538	1269.801964	13.747930
21.198219	1263.797936	13.752935
20.796097	1274.181778	13.757939
21.034419	1267.935246	13.762944
21.035910	1287.880541	13.767949
20.993308	1270.300973	13.772954
20.861265	1265.490213	13.777959
21.024476	1268.712747	13.782963
21.225226	1266.613331	13.787968
20.897132	1274.079010	13.792973
21.055872	1275.484013	13.797978
21.144085	1264.685059	13.802983
20.993863	1276.370723	13.807987
21.012192	1274.486485	13.812992
21.034578	1277.502824	13.817997
20.998829	1274.088090	13.823002
20.926082	1270.267669	13.828007
20.559687	1269.482445	13.833011
20.970036	1262.811079	13.838016
20.984223	1289.297195	13.843021
20.902791	1283.905916	13.848026
21.256842	1277.839618	13.853031
21.145395	1277.419008	13.858035
21.087788	1282.572287	13.863040
20.907802	1277.983638	13.868045
21.221405	1275.511401	13.873050
21.066859	1272.882023	13.878055
21.154364	1281.566645	13.883059
21.118111	1281.370587	13.888064
21.067732	1265.754017	13.893069
21.054311	1267.787306	13.898074
20.947908	1265.861464	13.903079
20.827859	1273.565197	13.908083
21.050289	1268.074991	13.913088
20.702453	1280.903942	13.918093
21.045597	1283.998430	13.923098
20.840492	1281.870708	13.928103
21.111167	1279.384817	13.933107
21.306395	1266.012523	13.938112
21.240488	1281.288116	13.943117
20.861318	1276.535695	13.948122
21.179534	1259.709149	13.953127
20.806519	1254.224040	13.958131
20.838062	1254.412987	13.963136
20.927508	1282.251164	13.968141
21.166854	1283.045638	13.973146
21.137077	1285.311776	13.978151
20.746340	1284.584051	13.983155
20.978917	1272.312828	13.988160
20.926806	1281.413963	13.993165
20.590589	1295.050059	13.998170
20.970323	1283.211099	14.003175
20.762924	1283.332503	14.008179
20.848060	1282.104667	14.013184
20.979780	1276.578464	14.018189
21.195980	1285.851923	14.023207
21.687965	1278.805299	14.028224
21.108350	1285.394040	14.033242
21.304457	1276.091816	14.038259
21.334650	1268.409458	14.043277
20.901728	1258.425827	14.048295
20.981455	1266.293580	14.053312
21.125072	1276.527870	14.058330
21.331899	1270.572745	14.063347
20.939825	1281.952652	14.068365
20.734505	1282.175741	14.073383
21.157810	1276.341806	14.078400
21.128654	1287.572597	14.083418
21.349674	1291.944757	14.088435
21.497218	1279.089121	14.093453
21.070395	1289.249251	14.098471
21.297075	1274.026293	14.103488
21.159809	1283.773735	14.108506
21.185915	1276.162807	14.113523
20.987806	1294.841721	14.118541
20.984308	1289.234728	14.123559
21.191096	1278.439644	14.128576
20.882573	1297.905345	14.133594
20.837354	1291.845704	14.138611
21.131922	1290.073204	14.143629
20.902982	1319.961187	14.148647
21.230021	1320.412378	14.153664
21.310997	1332.509636	14.158682
21.365105	1320.425459	14.163699
21.298787	1314.501302	14.168717
21.484634	1314.622673	14.173735
21.741139	1317.878676	14.178752
21.132705	1308.138501	14.183770
21.388227	1332.472220	14.188787
21.678124	1332.882147	14.193805
21.573390	1339.862331	14.198823
21.879472	1346.358584	14.203840
21.617037	1341.291500	14.208858
21.654054	1318.372399	14.213875
21.430735	1354.434966	14.218893
21.571063	1334.148219	14.223911
21.743299	1378.155660	14.228928
21.615170	1369.161488	14.233946
22.020888	1358.147432	14.238963
21.919315	1364.011897	14.243981
21.723745	1366.599159	14.248999
22.218662	1363.684186	14.254016
22.042832	1358.400370	14.259034
21.931869	1342.985816	14.264051
21.441542	1337.945646	14.269069
21.468386	1362.273421	14.274087
22.056582	1360.048255	14.279104
22.000418	1359.552306	14.284122
21.792770	1373.093994	14.289139
22.415417	1361.524685	14.294157
21.981867	1372.076038	14.299175
21.875248	1368.445368	14.304192
21.717644	1378.397455	14.309210
21.848040	1368.262549	14.314227
21.800059	1370.060239	14.319245
21.849581	1374.720890	14.324263
22.284027	1358.135555	14.329280
21.813096	1377.575360	14.334298
22.066399	1377.113415	14.339315
22.257337	1356.055681	14.344333
21.902896	1370.404113	14.349351
21.865574	1370.743545	14.354368
21.750816	1358.631218	14.359386
21.829403	1391.488798	14.364403
22.325214	1371.302593	14.369421
21.840025	1389.083645	14.374439
22.143849	1386.759122	14.379456
22.079362	1392.751385	14.384474
22.119479	1393.297106	14.389491
22.402110	1382.680176	14.394509
22.093799	1387.127359	14.399527
22.496665	1391.456387	14.404544
22.633269	1387.832531	14.409562
22.286563	1378.215721	14.414579
22.455190	1381.168019	14.419597
22.349043	1400.084073	14.424615
22.607178	1383.731316	14.429632
22.446825	1384.381370	14.434650
22.424081	1395.689871	14.439667
22.434550	1398.304046	14.444685
22.728204	1388.127355	14.449703
22.529338	1372.445231	14.454720
22.250724	1400.458472	14.459738
22.391872	1389.950617	14.464755
22.676808	1404.002050	14.469773
22.677215	1416.964775	14.474791
22.943408	1414.114589	14.479808
22.474709	1417.926721	14.484826
22.497046	1414.802412	14.489843
22.995432	1413.982062	14.494861
22.593121	1413.928273	14.499879
22.910983	1417.272036	14.504896
22.839072	1416.147839	14.509914
22.729284	1422.214978	14.514931
23.146052	1421.399781	14.519949
22.771561	1417.149609	14.524967
22.869340	1420.929583	14.529984
23.145547	1417.599618	14.535002
23.092566	1415.953324	14.540019
22.995368	1393.148319	14.545037
22.850946	1389.249979	14.550055
22.451474	1398.362948	14.555072
23.192426	1419.361782	14.560090
23.108782	1424.995333	14.565107
23.313630	1415.921279	14.570125
22.818495	1407.139774	14.575143
23.050494	1401.002837	14.580160
23.484475	1398.596205	14.585178
22.631451	1409.271121	14.590195
22.988636	1387.316975	14.595213
23.370190	1416.594993	14.600231
23.008254	1419.032629	14.605248
23.179761	1426.192152	14.610266
22.916320	1425.093786	14.615283
23.302525	1415.490602	14.620301
23.000827	1424.606868	14.625319
23.185164	1422.123654	14.630336
22.951519	1423.628509	14.635354
22.948480	1429.568516	14.640371
23.258522	1421.498532	14.645389
23.225122	1433.036841	14.650407
23.524950	1425.751821	14.655424
23.479085	1423.118143	14.660442
23.346509	1414.738108	14.665459
23.682317	1427.623749	14.670477
23.311000	1424.684920	14.675495
23.568140	1418.411836	14.680512
23.410548	1419.774003	14.685530
23.390439	1428.315268	14.690547
23.703731	1426.341572	14.695565
23.736223	1422.523538	14.700583
23.450920	1421.490005	14.705600
23.392133	1409.050969	14.710618
23.420080	1421.913356	14.715635
23.619008	1419.361750	14.720653
23.403349	1422.998246	14.725671
23.651207	1422.219430	14.730688
23.887414	1412.158847	14.735706
23.740062	1415.145824	14.740723
23.758933	1407.477782	14.745741
23.560359	1413.389199	14.750759
23.664118	1419.128130	14.755776
23.886661	1417.527546	14.760794
23.569097	1416.398490	14.765811
23.932420	1416.980744	14.770829
23.687879	1420.300963	14.775847
23.621247	1428.319559	14.780864
24.230974	1436.338810	14.785882
23.853148	1437.136808	14.790899
24.304989	1428.487373	14.795917
24.001446	1422.030026	14.800935
23.593507	1424.377476	14.805952
23.732179	1428.641695	14.810970
24.055960	1449.958790	14.815987
24.352425	1440.426530	14.821005
24.165145	1446.364473	14.826023
24.182898	1433.044931	14.831040
24.294340	1414.900338	14.836058
23.781902	1427.432089	14.841075
24.263090	1418.394176	14.846093
24.220008	1411.542944	14.851111
23.788793	1411.201195	14.856128
24.118016	1427.944790	14.861146
24.169295	1437.291041	14.866163
24.321301	1445.839467	14.871181
24.311544	1454.611894	14.876199
24.254219	1453.425595	14.881216
24.666294	1446.259508	14.886234
24.264233	1447.044070	14.891251
24.183076	1441.562658	14.896269
24.219453	1441.652819	14.901287
24.259394	1452.260833	14.906304
24.533599	1449.519469	14.911322
24.407490	1463.172500	14.916339
24.664002	1445.611894	14.921357
24.537337	1449.086343	14.926375
24.349955	1455.178455	14.931392
24.760569	1446.554462	14.936410
24.525053	1454.563833	14.941427
24.636593	1431.373127	14.946445
24.448043	1434.338365	14.951463
24.514346	1431.938468	14.956480
24.616995	1450.380853	14.961498
24.205587	1450.636816	14.966515
24.665101	1441.382131	14.971533
24.709279	1451.692179	14.976551
24.292587	1458.728471	14.981568
24.578583	1441.795500	14.986586
24.481513	1449.405273	14.991603
24.818043	1433.041530	14.996621
24.706225	1444.630107	15.001639
24.708452	1438.918327	15.006656
24.613829	1433.023803	15.011674
24.652656	1446.543548	15.016691
24.666686	1435.192378	15.021709
24.802067	1444.444998	15.026727
24.499761	1454.476845	15.031744
25.074666	1450.372518	15.036762
25.138910	1463.337686	15.041779
25.298391	1463.011823	15.046797
24.882843	1463.413159	15.051815
24.955887	1455.698700	15.056832
25.437823	1451.656390	15.061850
24.968587	1450.145698	15.066867
24.894990	1440.556067	15.071885
25.183965	1448.495931	15.076903
25.195493	1456.852848	15.081920
25.500469	1449.120272	15.086938
25.413038	1444.572629	15.091955
25.208187	1423.258616	15.096973
24.992092	1431.225552	15.101991
25.110379	1427.198784	15.107008
25.366396	1429.979857	15.112026
25.112100	1441.954513	15.117043
25.328786	1449.231106	15.122061
25.336963	1452.869657	15.127079
24.999870	1445.818350	15.132096
25.514154	1450.308942	15.137114
25.506376	1462.204969	15.142131
25.394554	1464.003417	15.147149
25.713420	1465.836982	15.152167
25.223747	1461.009014	15.157184
25.176737	1458.883581	15.162202
25.216549	1463.566258	15.167219
25.619639	1461.447678	15.172237
25.978953	1461.991250	15.177255
25.548152	1474.481707	15.182272
25.977619	1464.234538	15.187290
25.407669	1456.150750	15.192307
25.568622	1463.389051	15.197325
25.906107	1462.724920	15.202343
25.688938	1453.950956	15.207360
25.767106	1455.615282	15.212378
25.553284	1455.238856	15.217395
25.613438	1463.381961	15.222413
25.726261	1451.717729	15.227431
25.441140	1476.112759	15.232448
25.693923	1476.448390	15.237466
25.650026	1467.159159	15.242483
25.799498	1463.633903	15.247501
25.906576	1461.899154	15.252519
25.760130	1468.407871	15.257536
25.723687	1457.618420	15.262554
25.888537	1458.954326	15.267571
25.671083	1465.304487	15.272589
25.971247	1468.539405	15.277607
25.460294	1473.912383	15.282624
25.567182	1466.343525	15.287642
25.937967	1485.013734	15.292659
26.219347	1499.567605	15.297677
26.108627	1503.369848	15.302695
26.144949	1494.973836	15.307712
26.297650	1492.678121	15.312730
26.406678	1495.336365	15.317747
26.348195	1495.902537	15.322765
26.570740	1480.835747	15.327783
26.291615	1481.451269	15.332800
26.419518	1466.530146	15.337818
26.240267	1465.196560	15.342835
26.139285	1462.813903	15.347853
26.238906	1457.684308	15.352871
26.397909	1474.002093	15.357888
26.488754	1484.619314	15.362906
26.325692	1482.020049	15.367923
26.423012	1485.276315	15.372941
26.940359	1485.134033	15.377959
26.444287	1477.751004	15.382976
26.409292	1458.645035	15.387994
26.319966	1467.986993	15.393011
26.570061	1468.725732	15.398029
26.514884	1481.423684	15.403047
26.519077	1493.547482	15.408064
26.498071	1489.978628	15.413082
26.744098	1493.206456	15.418099
26.475130	1494.348877	15.423117
26.861096	1491.246772	15.428135
26.535925	1500.407726	15.433152
26.506652	1500.794639	15.438170
26.743440	1486.188026	15.443187
26.740944	1496.201966	15.448205
27.016817	1493.391118	15.453223
26.620981	1498.201495	15.458240
26.416645	1493.246209	15.463258
26.545921	1497.058930	15.468275
26.499109	1490.960136	15.473293
26.870500	1486.677483	15.478311
27.042914	1497.369789	15.483328
26.899260	1486.177433	15.488346
27.070070	1484.607116	15.493363
27.176420	1501.117368	15.498381
27.162932	1483.709891	15.503399
26.903601	1491.064006	15.508416
27.216764	1489.299528	15.513434
27.410373	1488.692951	15.518451
27.138320	1490.834700	15.523469
27.472542	1485.324767	15.528487
27.095494	1494.723646	15.533504
26.999564	1492.031876	15.538522
27.241818	1493.633855	15.543539
27.012893	1501.444006	15.548557
27.166104	1484.909678	15.553575
26.959841	1498.789451	15.558592
27.151729	1490.994670	15.563610
27.080863	1491.956060	15.568627
27.015880	1514.614086	15.573645
27.705616	1525.096486	15.578663
27.559840	1518.343378	15.583680
27.560338	1511.577953	15.588698
27.495372	1504.824545	15.593715
27.563263	1496.347994	15.598733
27.778816	1489.430304	15.603751
27.309285	1503.046917	15.608768
27.275707	1496.488275	15.613786
27.658452	1508.064082	15.618803
27.609123	1527.817498	15.623821
27.925063	1529.195376	15.628839
27.851150	1520.080781	15.633856
27.310063	1504.983192	15.638874
27.507195	1499.038959	15.643891
27.505607	1513.799995	15.648909
27.965769	1523.172315	15.653927
27.764439	1522.229196	15.658944
27.987281	1515.288309	15.663962
27.974030	1522.007031	15.668979
28.014704	1527.833144	15.673997
28.048583	1524.364062	15.679015
27.940514	1510.677566	15.684032
27.858605	1495.311697	15.689050
27.944522	1512.172848	15.694067
27.761997	1517.021563	15.699085
27.834037	1507.156982	15.704103
27.878508	1536.614848	15.709120
28.090089	1525.921060	15.714138
28.447889	1516.525254	15.719155
28.072402	1532.126144	15.724173
28.052324	1532.049136	15.729191
28.384034	1529.123986	15.734208
28.104554	1529.047457	15.739226
27.892337	1526.232662	15.744243
28.027421	1535.941550	15.749261
28.106016	1519.818619	15.754279
27.895977	1522.274513	15.759296
28.221610	1524.884057	15.764314
28.570379	1520.601856	15.769331
28.069064	1528.497940	15.774349
28.010352	1519.613720	15.779367
28.093377	1521.267841	15.784384
28.004448	1525.109084	15.789402
28.249197	1524.156158	15.794419
28.044293	1542.095603	15.799437
28.368059	1546.309884	15.804455
28.309912	1552.488386	15.809472
28.259764	1551.444075	15.814490
28.784130	1541.902138	15.819507
28.568767	1552.425110	15.824525
28.695222	1543.372919	15.829543
29.046556	1547.450673	15.834560
28.648112	1546.406863	15.839578
28.858110	1547.910177	15.844595
28.587555	1555.122974	15.849613
28.744976	1540.783787	15.854631
28.945137	1559.638607	15.859648
28.541546	1552.926606	15.864666
28.923909	1545.496232	15.869683
28.736210	1559.406134	15.874701
28.593888	1541.295568	15.879719
28.670280	1549.326023	15.884736
28.746611	1550.101921	15.889754
29.030210	1551.508555	15.894771
28.810376	1550.437828	15.899789
29.261024	1549.744633	15.904807
29.094128	1550.499554	15.909824
29.250248	1549.151790	15.914842
29.213071	1545.594940	15.919859
29.175233	1549.162206	15.924877
29.130914	1557.652354	15.929895
29.131165	1542.690168	15.934912
28.875887	1554.916750	15.939930
28.997611	1548.136690	15.944947
29.033250	1555.468956	15.949965
28.923735	1556.216297	15.954983
29.395193	1548.480709	15.960000
28.798022	1559.578950	15.965018
29.566131	1568.872294	15.970035
29.453999	1582.155130	15.975053
29.483337	1575.772027	15.980071
29.526533	1583.898243	15.985088
29.347681	1570.933182	15.990106
29.472187	1557.489535	15.995123
29.239697	1571.920957	16.000141
29.294097	1586.335733	16.005159
29.628046	1577.575245	16.010176
29.331869	1592.997600	16.015194
29.556039	1591.393592	16.020211
29.592649	1591.134515	16.025229
29.299778	1591.752233	16.030247
29.583193	1590.989759	16.035264
29.309966	1591.229974	16.040282
29.737681	1588.553760	16.045299
29.872585	1582.619419	16.050317
29.594314	1589.276628	16.055335
29.736294	1586.090728	16.060352
29.560936	1588.646491	16.065370
29.884422	1576.148697	16.070387
30.036529	1589.453097	16.075405
29.911622	1586.583466	16.080423
29.795389	1579.142157	16.085440
29.859408	1581.433227	16.090458
29.745565	1574.044235	16.095475
29.645277	1603.664536	16.100493
30.124605	1604.824457	16.105511
30.640313	1596.169456	16.110528
30.166603	1605.083615	16.115546
30.194581	1593.413927	16.120563
30.205669	1584.070235	16.125581
29.968089	1579.275159	16.130599
30.369028	1587.784750	16.135616
30.308438	1591.541268	16.140634
30.038105	1572.699982	16.145651
30.462001	1590.506943	16.150669
30.275705	1598.613931	16.155687
30.729815	1590.234593	16.160704
30.149456	1590.542674	16.165722
30.574267	1572.679012	16.170739
30.381555	1588.058117	16.175757
30.396346	1576.778286	16.180775
30.487757	1565.727694	16.185792
30.147204	1593.284798	16.190810
30.389444	1594.915105	16.195827
30.426455	1608.740449	16.200845
30.357166	1613.432712	16.205863
30.620625	1597.607389	16.210880
30.459641	1607.769379	16.215898
30.633956	1613.138493	16.220915
30.851367	1600.965116	16.225933
30.665103	1609.023342	16.230951
30.644168	1602.896778	16.235968
30.819640	1605.289622	16.240986
30.984131	1593.709841	16.246003
30.766804	1601.080906	16.251021
30.832523	1605.693432	16.256039
31.129776	1610.907659	16.261056
30.976019	1607.669828	16.266074
30.674905	1606.078821	16.271091
30.815428	1608.774533	16.276109
30.660877	1606.740162	16.281127
30.681844	1605.693941	16.286144
30.726671	1611.349543	16.291162
30.952780	1606.813183	16.296179
31.024594	1614.435430	16.301197
30.738463	1625.650844	16.306215
31.195784	1619.754721	16.311232
31.066014	1632.821771	16.316250
31.109625	1637.873551	16.321267
31.363635	1629.019606	16.326285
30.958864	1638.776921	16.331303
31.611278	1632.374632	16.336320
31.521869	1632.041275	16.341338
31.512429	1623.191604	16.346355
31.621809	1628.995787	16.351373
31.440942	1630.098997	16.356391
31.699437	1625.470952	16.361408
31.367220	1622.027208	16.366426
31.049300	1617.736492	16.371443
31.542465	1617.528857	16.376461
31.727422	1631.266133	16.381479
31.791822	1621.961102	16.386496
31.754342	1631.106136	16.391514
31.530384	1621.584412	16.396531
31.564669	1619.950916	16.401549
31.712324	1631.432190	16.406567
32.176118	1630.427017	16.411584
31.657945	1624.662892	16.416602
31.594506	1622.939593	16.421619
32.038502	1611.522850	16.426637
31.755891	1630.871608	16.431655
31.910457	1624.536148	16.436672
31.742001	1637.445783	16.441690
32.029271	1627.177138	16.446707
31.864177	1625.197927	16.451725
31.531805	1628.109068	16.456743
31.949319	1616.410261	16.461760
31.753403	1621.948541	16.466778
31.915072	1626.891826	16.471795
32.208320	1618.586892	16.476813
32.008849	1628.286286	16.481831
32.259842	1622.781712	16.486848
31.977600	1623.204259	16.491866
32.516122	1613.052847	16.496883
32.743174	1620.560676	16.501901
32.227133	1631.153686	16.506919
32.546887	1618.197925	16.511936
32.135466	1622.107935	16.516954
31.929748	1620.457666	16.521971
32.117284	1622.941394	16.526989
32.113317	1632.735446	16.532007
32.165862	1615.679064	16.537024
32.196262	1624.828998	16.542042
32.139299	1625.536501	16.547059
32.690475	1640.294440	16.552077
32.242412	1655.641202	16.557095
33.052002	1646.196846	16.562112
32.670121	1657.996979	16.567130
32.448068	1656.607282	16.572147
33.053105	1647.307234	16.577165
32.729640	1642.841220	16.582183
32.459437	1632.367343	16.587200
32.651578	1651.138620	16.592218
32.876386	1651.027271	16.597235
32.860525	1651.904394	16.602253
32.787013	1656.871044	16.607271
32.823380	1645.961302	16.612288
32.684135	1650.117335	16.617306
32.894382	1651.252542	16.622323
32.776724	1650.863917	16.627341
32.915865	1650.759939	16.632359
33.024004	1647.426844	16.637376
32.703007	1646.567297	16.642394
32.629936	1650.865355	16.647411
33.049674	1645.598119	16.652429
33.139296	1647.056152	16.657447
33.211181	1654.573018	16.662464
32.803878	1652.240762	16.667482
32.673832	1651.029867	16.672499
33.096776	1672.742025	16.677517
33.104558	1673.307072	16.682535
33.208888	1679.417242	16.687552
33.559606	1672.202632	16.692570
33.651918	1681.828780	16.697587
33.982695	1674.217811	16.702605
33.831574	1681.674309	16.707623
33.819208	1661.339102	16.712640
33.478090	1637.087716	16.717658
33.604819	1642.321290	16.722675
33.871091	1635.711611	16.727693
33.728662	1644.692500	16.732711
33.493228	1641.532182	16.737728
33.771661	1642.211357	16.742746
33.555671	1635.304229	16.747763
33.460803	1632.220590	16.752781
33.268498	1648.201361	16.757799
33.553921	1660.327631	16.762816
33.682880	1669.529510	16.767834
33.460496	1675.984367	16.772851
33.801914	1671.840146	16.777869
33.248260	1670.847823	16.782887
33.460598	1672.489200	16.787904
33.871685	1672.986773	16.792922
34.122477	1675.141104	16.797939
34.207545	1671.254845	16.802957
33.683408	1676.963472	16.807975
33.927335	1676.048421	16.812992
34.102673	1660.285848	16.818010
34.349405	1671.038786	16.823027
34.395570	1662.425608	16.828045
34.207824	1677.620763	16.833063
33.977279	1674.398311	16.838080
34.529379	1665.728027	16.843098
33.973948	1672.320945	16.848115
34.353690	1671.335468	16.853133
34.300654	1678.335882	16.858151
34.535822	1669.878166	16.863168
35.206459	1665.278750	16.868186
35.002397	1663.560573	16.873203
35.269707	1651.709521	16.878221
35.081648	1655.130892	16.883239
35.088004	1637.040534	16.888256
34.882201	1622.041920	16.893274
34.958834	1622.366327	16.898291
34.970617	1613.195533	16.903309
34.809266	1622.681210	16.908327
34.844126	1620.176188	16.913344
34.807011	1607.952169	16.918362
34.745325	1623.161766	16.923379
34.701423	1616.323151	16.928397
34.823197	1619.270388	16.933415
34.667102	1614.669150	16.938432
34.532850	1621.054871	16.943450
34.703210	1610.384898	16.948467
34.986253	1612.653623	16.953485
34.951628	1616.248707	16.958503
34.856152	1612.860010	16.963520
35.148604	1608.220262	16.968538
34.883682	1615.451066	16.973555
34.794681	1616.945451	16.978573
34.981501	1641.336267	16.983591
35.067368	1639.913186	16.988608
35.318959	1640.859331	16.993626
35.191187	1650.894934	16.998643
35.065870	1644.965895	17.003661
35.387724	1649.653981	17.008679
35.553479	1648.413208	17.013696
35.586794	1645.801466	17.018714
35.304023	1651.910448	17.023731
35.429535	1650.419696	17.028749
35.506387	1649.188384	17.033767
35.416418	1648.476026	17.038784
35.538672	1642.125263	17.043802
35.067709	1650.523072	17.048819
35.591036	1636.476204	17.053837
35.382647	1644.986281	17.058855
35.475634	1656.042150	17.063872
35.742362	1642.626075	17.068890
35.438154	1645.705755	17.073907
35.452076	1644.314599	17.078925
35.464244	1643.131356	17.083943
35.330483	1635.301926	17.088960
36.070425	1661.617974	17.093978
35.881452	1666.422150	17.098995
35.982258	1669.305103	17.104013
36.005873	1664.247332	17.109031
36.100364	1674.250646	17.114048
36.180263	1647.586759	17.119066
35.716298	1661.295438	17.124083
36.019456	1663.702531	17.129101
36.008208	1661.264631	17.134119
36.119361	1665.613532	17.139136
36.192551	1665.032447	17.144154
36.056621	1675.182623	17.149171
36.316011	1665.538157	17.154189
35.902239	1668.094209	17.159207
35.737252	1668.392664	17.164224
36.071827	1670.953619	17.169242
36.019206	1672.426478	17.174259
35.837796	1673.119227	17.179277
36.296096	1676.786710	17.184295
36.472195	1691.711492	17.189312
36.684941	1692.742486	17.194330
36.724005	1708.357664	17.199347
36.697637	1704.339736	17.204365
37.056834	1697.760824	17.209383
36.531302	1685.973285	17.214400
36.571042	1676.075989	17.219418
36.474084	1672.483026	17.224435
36.696025	1692.643274	17.229453
36.801600	1689.524506	17.234471
37.068844	1694.922872	17.239488
37.252092	1690.445233	17.244506
37.045064	1679.745743	17.249523
36.557067	1669.863415	17.254541
36.545771	1678.518249	17.259559
36.519312	1695.454166	17.264576
36.917482	1691.047636	17.269594
36.562468	1700.082917	17.274611
36.739528	1693.959339	17.279629
36.761615	1701.013848	17.284647
36.609312	1709.030534	17.289664
37.166777	1708.166142	17.294682
36.900157	1728.983230	17.299699
37.311776	1732.365596	17.304717
37.413783	1730.980830	17.309735
37.466721	1719.454921	17.314752
37.366859	1734.953863	17.319770
37.626782	1723.281681	17.324787
37.445679	1741.873514	17.329805
37.435422	1728.136605	17.334823
37.415657	1738.603345	17.339840
37.794054	1726.201269	17.344858
37.587266	1704.117954	17.349875
37.750855	1715.958543	17.354893
37.922242	1696.391486	17.359911
37.184143	1691.979007	17.364928
37.595019	1705.058987	17.369946
37.734749	1727.335490	17.374963
37.715038	1725.474645	17.379981
37.964274	1716.527029	17.384999
37.888973	1713.179134	17.390016
37.889863	1700.920661	17.395034
37.754060	1708.426638	17.400051
38.203465	1709.663700	17.405069
38.189621	1694.014634	17.410087
37.890371	1698.145867	17.415104
37.733595	1688.449790	17.420122
37.831172	1699.899782	17.425139
37.979617	1715.094835	17.430157
37.968669	1719.548169	17.435175
38.106298	1714.396691	17.440192
38.311630	1708.296912	17.445210
37.991314	1728.427300	17.450227
38.148053	1721.260910	17.455245
38.193922	1717.995932	17.460263
37.955034	1721.280709	17.465280
37.973708	1710.241609	17.470298
38.092156	1726.803672	17.475315
37.963868	1721.697752	17.480333
38.235870	1730.911461	17.485351
38.521013	1749.601968	17.490368
38.500368	1757.728240	17.495386
38.589070	1754.462713	17.500403
38.531654	1748.505498	17.505421
38.670753	1746.026300	17.510439
38.782243	1752.316253	17.515456
38.770605	1749.242908	17.520474
38.606079	1748.838161	17.525491
38.710568	1752.266374	17.530509
38.847136	1746.273499	17.535527
38.849758	1753.433383	17.540544
38.906700	1745.636396	17.545562
39.098910	1744.726444	17.550579
38.800049	1736.020392	17.555597
39.031065	1732.640938	17.560615
38.695542	1736.625385	17.565632
38.471435	1737.106301	17.570650
39.039678	1730.943908	17.575667
39.199353	1760.962719	17.580685
39.463614	1761.092038	17.585703
39.170987	1751.510395	17.590720
39.294800	1746.475938	17.595738
39.190482	1738.111656	17.600755
38.992676	1744.048252	17.605773
39.429977	1748.936604	17.610791
39.586427	1755.680277	17.615808
39.703596	1749.693641	17.620826
39.602535	1744.965609	17.625843
39.298658	1742.632570	17.630861
39.798704	1739.394244	17.635879
39.782168	1737.620979	17.640896
39.499606	1732.379216	17.645914
39.464645	1729.134993	17.650931
39.475712	1743.090445	17.655949
40.035467	1738.774530	17.660967
39.733176	1746.281913	17.665984
39.587069	1749.803578	17.671002
39.847541	1743.430726	17.676019
39.762466	1749.991126	17.681037
40.057595	1749.884291	17.686055
39.888457	1754.015234	17.691072
39.680407	1750.981082	17.696090
40.010866	1745.098852	17.701107
39.620245	1752.967961	17.706125
40.237394	1749.857244	17.711143
39.927674	1742.905240	17.716160
39.931840	1746.500461	17.721178
40.190360	1749.207267	17.726195
40.007238	1747.586411	17.731213
40.365757	1751.845548	17.736231
40.305526	1748.927815	17.741248
40.098740	1752.548820	17.746266
40.276487	1752.739128	17.751283
39.970915	1751.746553	17.756301
40.515866	1757.619739	17.761319
40.571383	1769.126830	17.766336
40.414322	1775.774228	17.771354
40.784553	1780.657560	17.776371
40.583190	1787.080798	17.781389
41.027459	1778.970333	17.786407
40.758114	1778.190626	17.791424
40.636866	1782.005630	17.796442
40.851688	1771.330021	17.801459
40.531398	1785.289602	17.806477
41.016967	1770.932454	17.811495
40.813731	1769.173234	17.816512
40.671031	1777.326850	17.821530
40.834916	1774.032025	17.826547
40.545404	1780.541678	17.831565
40.876513	1771.228617	17.836583
40.479102	1775.913494	17.841600
40.675588	1788.120124	17.846618
41.135880	1790.020837	17.851635
40.805282	1804.902287	17.856653
41.003692	1805.624122	17.861671
41.513141	1802.843600	17.866688
41.107744	1811.053292	17.871706
41.317879	1808.704324	17.876723
41.479020	1813.241922	17.881741
41.776680	1798.283944	17.886759
41.506124	1804.233741	17.891776
41.638895	1806.447815	17.896794
41.864452	1802.776637	17.901811
41.784596	1802.652534	17.906829
41.767732	1781.783054	17.911847
41.267516	1770.793638	17.916864
41.339025	1785.010045	17.921882
41.645309	1786.375334	17.926899
41.702419	1801.591338	17.931917
41.629247	1797.462873	17.936935
41.467563	1802.542736	17.941952
41.657605	1798.801719	17.946970
41.645468	1798.934226	17.951987
41.678442	1802.963734	17.957005
41.900364	1797.451148	17.962023
41.907998	1800.690331	17.967040
41.401505	1800.436079	17.972058
41.884581	1800.881277	17.977075
42.038666	1825.905254	17.982093
42.337377	1821.602638	17.987111
42.218318	1831.896522	17.992128
42.162547	1830.791739	17.997146
42.535390	1818.253619	18.002163
42.230076	1837.680205	18.007181
42.361331	1827.497651	18.012199
42.481578	1831.546281	18.017216
42.441996	1832.851910	18.022234
42.766940	1813.294810	18.027251
42.695985	1826.623211	18.032269
42.816349	1814.575244	18.037287
42.795584	1815.534955	18.042304
42.643918	1801.759184	18.047322
42.682450	1798.592884	18.052339
42.887860	1792.386093	18.057357
42.852743	1779.579599	18.062375
42.611730	1776.276996	18.067392
42.511435	1796.100255	18.072410
42.913641	1805.198865	18.077427
42.890278	1819.891329	18.082445
42.903565	1814.564596	18.087463
42.945402	1813.738399	18.092480
42.901928	1819.716475	18.097498
43.218081	1802.458954	18.102515
43.013681	1809.804467	18.107533
43.288676	1802.254238	18.112551
43.351873	1803.349992	18.117568
43.074628	1803.512200	18.122586
43.352805	1811.957351	18.127603
43.038485	1805.839743	18.132621
43.406561	1794.406653	18.137639
43.484737	1804.645464	18.142656
43.286504	1807.546255	18.147674
43.449854	1803.840954	18.152691
43.060614	1808.378248	18.157709
43.257709	1807.423469	18.162727
43.140435	1808.887777	18.167744
43.324901	1824.619887	18.172762
43.566752	1842.796755	18.177779
43.638688	1840.449375	18.182797
43.707899	1838.557029	18.187815
43.592617	1841.900768	18.192832
43.643455	1849.479295	18.197850
43.886197	1834.468692	18.202867
44.041347	1845.637486	18.207885
43.825887	1834.228226	18.212903
44.055553	1836.581005	18.217920
43.996040	1838.695194	18.222938
43.991678	1835.619098	18.227955
43.798488	1838.224938	18.232973
44.102276	1834.807112	18.237991
43.867393	1843.028950	18.243008
43.691495	1834.128622	18.248026
44.103053	1848.657365	18.253043
44.268254	1864.191245	18.258061
44.486408	1865.619362	18.263079
44.428992	1863.331935	18.268096
44.319755	1878.333881	18.273114
44.601972	1869.640458	18.278131
44.349086	1861.054411	18.283149
44.590556	1860.219965	18.288167
44.375218	1860.867797	18.293184
44.350275	1871.830957	18.298202
44.724524	1869.418051	18.303219
44.658618	1867.748598	18.308237
44.429693	1870.614971	18.313255
44.456399	1863.326107	18.318272
44.559631	1860.094419	18.323290
45.007563	1873.395157	18.328307
45.115003	1891.952171	18.333325
45.096798	1871.889732	18.338343
45.296021	1870.165407	18.343360
45.104786	1868.580437	18.348378
45.282386	1864.105218	18.353395
45.140086	1858.177227	18.358413
45.192099	1856.627392	18.363431
45.068515	1848.056908	18.368448
44.900727	1866.052180	18.373466
45.244838	1877.466136	18.378483
45.135691	1891.105853	18.383501
45.458503	1894.381301	18.388519
45.808897	1882.807818	18.393536
45.246442	1893.848863	18.398554
45.495473	1886.456887	18.403571
45.329481	1879.687957	18.408589
45.128874	1882.507344	18.413607
45.827648	1884.341720	18.418624
45.372188	1888.787355	18.423642
45.620097	1891.668912	18.428659
45.727216	1887.447172	18.433677
45.771828	1895.887154	18.438695
45.913832	1876.771278	18.443712
45.775890	1881.383342	18.448730
45.874268	1881.833275	18.453747
45.883426	1890.110596	18.458765
45.931474	1897.017915	18.463783
46.145301	1909.906144	18.468800
46.124382	1915.995492	18.473818
46.456567	1911.196730	18.478835
46.327042	1889.583724	18.483853
46.061026	1889.865263	18.488871
46.122952	1895.338925	18.493888
46.025641	1917.985436	18.498906
46.476854	1917.751459	18.503923
46.398671	1924.884990	18.508941
46.454058	1925.571442	18.513959
46.675120	1910.353434	18.518976
46.811173	1910.053322	18.523994
46.736993	1908.671473	18.529011
46.548205	1910.724495	18.534029
46.425830	1913.789385	18.539047
46.863271	1911.157182	18.544064
46.581217	1923.492162	18.549082
46.605648	1912.302553	18.554099
46.720807	1902.021841	18.559117
46.464910	1910.237631	18.564135
46.678415	1911.369194	18.569152
46.623618	1910.009422	18.574170
46.643101	1901.419233	18.579187
46.416928	1930.724443	18.584205
46.505068	1940.565359	18.589223
47.095501	1931.449934	18.594240
47.143734	1942.977202	18.599258
47.325560	1934.551436	18.604275
47.477098	1945.077519	18.609293
47.127095	1939.130712	18.614311
47.216577	1932.242359	18.619328
47.279381	1932.713697	18.624346
47.106571	1935.047317	18.629363
47.068599	1951.055715	18.634381
47.352995	1970.909090	18.639399
47.852939	1948.280098	18.644416
47.591819	1966.855095	18.649434
47.895507	1966.051618	18.654451
48.077269	1968.747114	18.659469
48.157424	1969.870063	18.664487
48.068112	1966.923892	18.669504
47.923288	1940.322051	18.674522
48.047240	1933.867072	18.679539
47.863353	1923.591571	18.684557
47.761066	1943.978490	18.689575
48.478344	1939.840313	18.694592
48.092428	1939.318287	18.699610
48.248561	1939.210026	18.704627
48.111473	1924.154521	18.709645
48.262043	1943.495950	18.714663
48.311332	1949.750294	18.719680
48.375904	1964.686854	18.724698
48.435860	1951.105275	18.729715
47.962456	1941.088297	18.734733
48.282161	1955.205510	18.739751
48.465107	1951.209184	18.744768
48.381198	1951.096737	18.749786
48.053333	1955.688781	18.754803
48.562204	1955.050779	18.759821
48.488177	1960.783676	18.764839
48.622574	1955.646787	18.769856
47.986464	1954.582648	18.774874
48.366279	1955.999147	18.779891
48.865403	1971.355614	18.784909
48.859485	1979.207528	18.789927
49.200792	1967.945313	18.794944
49.171525	1981.786305	18.799962
49.298476	1976.910144	18.804979
49.714517	1977.326716	18.809997
49.530177	1953.038781	18.815015
49.315661	1952.429641	18.820032
49.240029	1953.247103	18.825050
48.844178	1950.629824	18.830067
49.021931	1943.481996	18.835085
48.892578	1955.893321	18.840103
49.618209	1955.028838	18.845120
49.714205	1963.990773	18.850138
49.654131	1957.154576	18.855155
49.822510	1943.393689	18.860173
49.352629	1956.197528	18.865191
49.718178	1957.190013	18.870208
49.836239	1954.764472	18.875226
49.874447	1954.541313	18.880243
49.839968	1940.764021	18.885261
49.259034	1952.835238	18.890279
49.724602	1965.156402	18.895296
49.733492	1972.615842	18.900314
49.833903	1979.786982	18.905331
49.789346	1971.483818	18.910349
49.571894	1972.872885	18.915367
49.432297	1967.740367	18.920384
49.743281	1984.054939	18.925402
49.875647	2007.714164	18.930419
50.103258	2008.299218	18.935437
50.449341	2014.297039	18.940455
50.616572	2014.523635	18.945472
50.681471	2006.923440	18.950490
50.798834	2009.229666	18.955507
50.964723	2010.265012	18.960525
50.884643	1990.877667	18.965543
50.565563	1968.678150	18.970560
50.781820	1985.243786	18.975578
50.364961	1972.812612	18.980595
50.560610	1981.414171	18.985613
50.323979	1998.390256	18.990631
50.177217	2009.009581	18.995648
50.975954	1999.033479	19.000666
50.789981	2009.056589	19.005683
50.875220	2008.602558	19.010701
51.046377	2010.228522	19.015719
51.043851	2008.042429	19.020736
51.041101	1996.400913	19.025754
51.157026	1999.662193	19.030771
51.087899	2007.766451	19.035789
50.937827	2005.031310	19.040807
51.049014	2001.999669	19.045824
51.273176	1993.117232	19.050842
50.987230	1999.088438	19.055859
51.300902	1996.641129	19.060877
51.263129	2022.144359	19.065895
51.242812	2027.321302	19.070912
51.494188	2031.089523	19.075930
51.316774	2030.594013	19.080947
51.512042	2026.303118	19.085965
51.395509	2032.756978	19.090983
51.259980	2022.682907	19.096000
51.663591	2037.043221	19.101018
51.686420	2044.201599	19.106035
52.213832	2052.231185	19.111053
52.114219	2044.068895	19.116071
52.477207	2040.383604	19.121088
52.369613	2017.371631	19.126106
52.164991	2026.257282	19.131123
52.433608	2010.029566	19.136141
51.886696	2014.620385	19.141159
51.864018	2025.823974	19.146176
52.175958	2023.554689	19.151194
52.199027	2040.146481	19.156211
52.308874	2041.596610	19.161229
52.355322	2042.361572	19.166247
52.286841	2055.607990	19.171264
52.694974	2034.955079	19.176282
52.450972	2050.848583	19.181299
52.767580	2036.609361	19.186317
52.521174	2039.000353	19.191335
52.631816	2039.245414	19.196352
52.768376	2036.961628	19.201370
52.613722	2042.389665	19.206387
52.719868	2044.549821	19.211405
52.895228	2031.237625	19.216423
52.804215	2038.211236	19.221440
53.131960	2036.491562	19.226458
53.110792	2057.653790	19.231475
53.336870	2050.773482	19.236493
53.015093	2051.019872	19.241511
52.988609	2054.517811	19.246528
53.675984	2060.217397	19.251546
53.497637	2075.826749	19.256563
53.439511	2061.137608	19.261581
53.744460	2069.466955	19.266599
53.504205	2050.287549	19.271616
53.300603	2035.580738	19.276634
53.218260	2046.562624	19.281651
53.661241	2052.716467	19.286669
53.766137	2060.445358	19.291687
53.475193	2069.082107	19.296704
53.858303	2049.608222	19.301722
54.325281	2063.494412	19.306739
53.904630	2071.486457	19.311757
53.910725	2061.138085	19.316775
53.849556	2064.529873	19.321792
54.004052	2059.564348	19.326810
53.593188	2066.202022	19.331827
53.808640	2064.399580	19.336845
54.044676	2052.230721	19.341863
53.990642	2060.732151	19.346880
54.312210	2052.455489	19.351898
53.935403	2056.474921	19.356915
54.136617	2061.552049	19.361933
54.605151	2079.203847	19.366951
54.246062	2079.644952	19.371968
54.828682	2087.318112	19.376986
54.596845	2090.896004	19.382003
54.599852	2079.104064	19.387021
54.952152	2086.722723	19.392039
54.861644	2095.377856	19.397056
54.941810	2076.896075	19.402074
54.673585	2081.722465	19.407091
54.778215	2083.733431	19.412109
54.786129	2081.649482	19.417127
54.737637	2081.754756	19.422144
55.128077	2078.123279	19.427162
55.119404	2070.556807	19.432179
55.118800	2072.806354	19.437197
55.095477	2083.763124	19.442215
54.897529	2083.753808	19.447232
55.157934	2075.077900	19.452250
54.994694	2072.692487	19.457267
54.870532	2080.904664	19.462285
55.062819	2084.812886	19.467303
54.844149	2091.707782	19.472320
55.424309	2088.417280	19.477338
55.099611	2101.654269	19.482355
55.469615	2119.191269	19.487373
55.987217	2118.839736	19.492391
55.589203	2123.142569	19.497408
55.946953	2123.733614	19.502426
55.852090	2130.413725	19.507443
55.902418	2113.053515	19.512461
55.923783	2119.982500	19.517479
55.952655	2129.008726	19.522496
56.493099	2119.769023	19.527514
56.066183	2115.199808	19.532531
56.201599	2109.755959	19.537549
56.670764	2117.890828	19.542567
56.517814	2123.180196	19.547584
56.725074	2110.529808	19.552602
56.588151	2120.927420	19.557619
56.585162	2119.444533	19.562637
56.773785	2110.537805	19.567655
56.553431	2110.184421	19.572672
56.895291	2112.810365	19.577690
56.778341	2108.866547	19.582707
56.907902	2117.192435	19.587725
56.915167	2081.802680	19.592743
56.501723	2094.784829	19.597760
56.730590	2095.932834	19.602778
57.148399	2104.728697	19.607795
56.486134	2110.163787	19.612813
56.912153	2101.620326	19.617831
56.505378	2120.416952	19.622848
56.834987	2110.989084	19.627866
56.382947	2111.418273	19.632883
56.650099	2130.489673	19.637901
57.093671	2134.540303	19.642919
56.991655	2144.708992	19.647936
57.088967	2143.114150	19.652954
56.990420	2145.577532	19.657971
57.125178	2170.523389	19.662989
57.540067	2166.600124	19.668007
57.427778	2173.964163	19.673024
57.523961	2174.079396	19.678042
57.653287	2166.843227	19.683059
57.881048	2179.468349	19.688077
57.909154	2167.610986	19.693095
57.755868	2173.406945	19.698112
58.059478	2172.759203	19.703130
58.161357	2166.694610	19.708147
58.273769	2164.265217	19.713165
58.238441	2165.243004	19.718183
58.230613	2168.642039	19.723200
58.294623	2174.640872	19.728218
58.215160	2165.333270	19.733235
58.252130	2173.112381	19.738253
58.342509	2172.226511	19.743271
58.264880	2180.959866	19.748288
58.610732	2191.016257	19.753306
59.127005	2186.573442	19.758323
58.664819	2179.094976	19.763341
58.835278	2167.096931	19.768359
58.625344	2182.791660	19.773376
58.969876	2181.377610	19.778394
59.086106	2182.963591	19.783411
58.911710	2185.226715	19.788429
59.358493	2189.322468	19.793447
58.992587	2179.253569	19.798464
59.009736	2175.425200	19.803482
58.945541	2180.948974	19.808499
59.277451	2179.065023	19.813517
59.393223	2185.019425	19.818535
59.288949	2180.236705	19.823552
59.487756	2176.725432	19.828570
59.364835	2189.173683	19.833587
59.146290	2182.397262	19.838605
59.440347	2172.959294	19.843623
59.482149	2183.215185	19.848640
59.378661	2174.792314	19.853658
59.531499	2183.370934	19.858675
59.493807	2178.132424	19.863693
59.726807	2173.026923	19.868711
59.393634	2188.066478	19.873728
59.585403	2178.073805	19.878746
59.523150	2205.148014	19.883763
59.582746	2209.264626	19.888781
59.899779	2210.329365	19.893799
59.930978	2215.831645	19.898816
59.948965	2211.957514	19.903834
60.035125	2202.769766	19.908851
59.948077	2231.896088	19.913869
60.124779	2238.610015	19.918887
60.061655	2242.510252	19.923904
60.427424	2240.767187	19.928922
60.606791	2238.545757	19.933939
60.370571	2245.075430	19.938957
60.579366	2238.680718	19.943975
60.843089	2242.140281	19.948992
60.483837	2242.801643	19.954010
60.866784	2244.426890	19.959027
60.724524	2240.859886	19.964045
61.138215	2248.566369	19.969063
60.976130	2264.014450	19.974080
61.168136	2259.790076	19.979098
61.074541	2253.522238	19.984115
61.338707	2258.760859	19.989133
61.656445	2262.438332	19.994151
61.543701	2260.688213	19.999168
61.544687	2244.608316	20.004186
61.663898	2231.883775	20.009203
61.325610	2228.945799	20.014221
61.654273	2224.643009	20.019239
61.609805	2232.118957	20.024256
61.507764	2242.320753	20.029274
61.839172	2246.106156	20.034291
61.608432	2252.902377	20.039309
62.139929	2253.580550	20.044327
61.917869	2258.247049	20.049344
61.897541	2254.865091	20.054362
61.991969	2255.196114	20.059379
61.876976	2265.426733	20.064397
62.318753	2258.752603	20.069415
61.710554	2263.060684	20.074432
61.718677	2255.763575	20.079450
62.049740	2245.375826	20.084467
61.662188	2254.619560	20.089485
61.820592	2268.240553	20.094503
62.254852	2270.507291	20.099520
62.149407	2273.618320	20.104538
62.681135	2281.298130	20.109555
62.609938	2275.383794	20.114573
62.713306	2269.517126	20.119591
62.540010	2268.882521	20.124608
62.055117	2279.867437	20.129626
62.735349	2290.339338	20.134643
62.331810	2310.331215	20.139661
62.707305	2311.007530	20.144679
62.901883	2310.238743	20.149696
62.938843	2305.787395	20.154714
63.004051	2298.953078	20.159731
63.008158	2312.436696	20.164749
63.483556	2316.065442	20.169767
63.425600	2332.953643	20.174784
63.575032	2335.677961	20.179802
63.932988	2321.293438	20.184819
63.856689	2305.961992	20.189837
64.030574	2303.480299	20.194855
63.887001	2292.100110	20.199872
63.584985	2304.006003	20.204890
63.828623	2287.692299	20.209907
63.659467	2294.253770	20.214925
63.769966	2297.180923	20.219943
63.697581	2295.514026	20.224960
63.578043	2319.976871	20.229978
64.300823	2321.109043	20.234995
64.238237	2340.113757	20.240013
64.324150	2334.976602	20.245031
64.239301	2330.149835	20.250048
64.039266	2327.158326	20.255066
64.132117	2329.880656	20.260083
63.830044	2333.299917	20.265101
64.029798	2328.364836	20.270119
64.252554	2346.141106	20.275136
64.172772	2359.356570	20.280154
64.622302	2353.195553	20.285171
64.766325	2357.994037	20.290189
64.914562	2360.081459	20.295207
65.166209	2356.132269	20.300224
65.039684	2355.661664	20.305242
65.387506	2359.087394	20.310259
65.141435	2368.281892	20.315277
65.143270	2350.914974	20.320295
65.450653	2350.699217	20.325312
65.246252	2361.669346	20.330330
65.688578	2349.281716	20.335347
65.533428	2348.090495	20.340365
65.585238	2345.636129	20.345383
65.782343	2344.719070	20.350400
65.743000	2349.326567	20.355418
65.879687	2348.095093	20.360435
65.157948	2348.045043	20.365453
65.477657	2348.750708	20.370471
65.610121	2342.893528	20.375488
65.241748	2347.556648	20.380506
65.682318	2340.280190	20.385523
66.001048	2370.639849	20.390541
66.129401	2377.136604	20.395559
66.203283	2375.534462	20.400576
65.904397	2371.666781	20.405594
66.193422	2366.201484	20.410611
66.103173	2380.577985	20.415629
66.311005	2367.082547	20.420647
66.293423	2371.787257	20.425664
66.060409	2377.117801	20.430682
66.536340	2367.707331	20.435699
66.343214	2364.041441	20.440717
66.357956	2367.536026	20.445735
66.731215	2388.764821	20.450752
66.611560	2407.276916	20.455770
66.805126	2406.824473	20.460787
66.609568	2409.292360	20.465805
66.568839	2407.425341	20.470823
67.128572	2400.870764	20.475840
66.777078	2406.898208	20.480858
66.974220	2402.254537	20.485875
67.009230	2415.456462	20.490893
67.335651	2423.145497	20.495911
67.466239	2421.359695	20.500928
67.354893	2433.405962	20.505946
67.599132	2430.890217	20.510963
67.197829	2432.772705	20.515981
67.276593	2423.774765	20.520999
67.463916	2413.186446	20.526016
67.383007	2429.331211	20.531034
67.689324	2445.437045	20.536051
68.078177	2457.742553	20.541069
68.229201	2466.637032	20.546087
68.514939	2455.135546	20.551104
68.083534	2430.362380	20.556122
68.264983	2436.024043	20.561139
68.180197	2451.919333	20.566157
68.235660	2448.831205	20.571175
68.457505	2445.953289	20.576192
68.330544	2453.488128	20.581210
68.701329	2444.180111	20.586227
68.744721	2439.784326	20.591245
68.415468	2454.974545	20.596263
68.564735	2446.934361	20.601280
68.457292	2446.941284	20.606298
68.672209	2436.189667	20.611315
68.486477	2445.811905	20.616333
68.666439	2446.378623	20.621351
69.047747	2448.074158	20.626368
68.922408	2471.521976	20.631386
68.989133	2473.417129	20.636403
69.376522	2465.898972	20.641421
69.114394	2465.117285	20.646439
69.311696	2462.684528	20.651456
69.125411	2471.918321	20.656474
69.448267	2462.971093	20.661491
69.718029	2462.207612	20.666509
69.344803	2465.632746	20.671527
69.887046	2454.975993	20.676544
69.716852	2456.974998	20.681562
69.779386	2461.545046	20.686579
70.004130	2459.179489	20.691597
69.875364	2446.174190	20.696615
70.165084	2445.792930	20.701632
70.051447	2463.756707	20.706650
70.141090	2461.547981	20.711667
70.057801	2464.148986	20.716685
70.069776	2451.015840	20.721703
70.118681	2455.415808	20.726720
70.328148	2482.319778	20.731738
70.144579	2486.210974	20.736755
70.126688	2477.910346	20.741773
70.176230	2491.143844	20.746791
70.444078	2477.359511	20.751808
70.707804	2484.520586	20.756826
70.566355	2501.755005	20.761843
71.044326	2513.774205	20.766861
71.042214	2512.185741	20.771879
70.890328	2512.164357	20.776896
70.919735	2504.462593	20.781914
70.905226	2504.510539	20.786931
71.062921	2520.449817	20.791949
71.096575	2506.314256	20.796967
71.252397	2518.966879	20.801984
71.029110	2502.197276	20.807002
71.155765	2514.948932	20.812019
71.611705	2537.081865	20.817037
71.545976	2542.470735	20.822055
71.738381	2545.013627	20.827072
71.542296	2551.943678	20.832090
71.525461	2548.165463	20.837107
71.595589	2536.332560	20.842125
71.458901	2542.677384	20.847143
71.651718	2550.721290	20.852160
71.983502	2563.775340	20.857178
72.116018	2560.299719	20.862195
72.408244	2570.827416	20.867213
72.433556	2566.882020	20.872231
72.835217	2561.028225	20.877248
72.620005	2561.414932	20.882266
72.535201	2566.309757	20.887283
72.885291	2558.979980	20.892301
73.000038	2572.629459	20.897319
73.196749	2563.752627	20.902336
73.100516	2559.017265	20.907354
73.219462	2555.281890	20.912371
73.252407	2533.648303	20.917389
72.778297	2536.809534	20.922407
72.955458	2524.482924	20.927424
73.000175	2534.003969	20.932442
72.989843	2549.769510	20.937459
73.509255	2549.232060	20.942477
73.105658	2547.215249	20.947495
73.195299	2554.811552	20.952512
73.467093	2552.204872	20.957530
73.511085	2546.903649	20.962547
73.551133	2562.274976	20.967565
73.590811	2552.485635	20.972583
73.362568	2545.668116	20.977600
73.572302	2556.255365	20.982618
73.359958	2581.689887	20.987635
73.966074	2574.718048	20.992653
73.872875	2571.508880	20.997671
74.143752	2596.016892	21.002688
74.063213	2585.873880	21.007706
74.104934	2580.338617	21.012723
74.271547	2566.848782	21.017741
74.152568	2580.653526	21.022759
74.124894	2579.825001	21.027776
74.463841	2596.735154	21.032794
74.119358	2603.133595	21.037811
74.591504	2610.526558	21.042829
74.608111	2612.421857	21.047847
74.476712	2602.173682	21.052864
74.434698	2609.599881	21.057882
74.710546	2636.376354	21.062899
75.199491	2634.242351	21.067917
74.847924	2639.122328	21.072935
75.347132	2633.687908	21.077952
75.510286	2640.139117	21.082970
75.466674	2634.062926	21.087987
75.733129	2627.306476	21.093005
76.202527	2631.522239	21.098023
75.984287	2619.340412	21.103040
75.935474	2600.320874	21.108058
75.663178	2599.002017	21.113075
75.930094	2590.322406	21.118093
75.733348	2594.568891	21.123111
75.782717	2600.718106	21.128128
76.040727	2610.431709	21.133146
75.839581	2620.120230	21.138163
75.970296	2614.479520	21.143181
76.037502	2615.650206	21.148199
76.020399	2614.728753	21.153216
75.981670	2613.501637	21.158234
76.325179	2617.382742	21.163251
76.252146	2636.284898	21.168269
76.213287	2643.830166	21.173287
76.335067	2657.852214	21.178304
76.430086	2649.953497	21.183322
76.277354	2659.777474	21.188339
76.614780	2655.728005	21.193357
76.843945	2662.605230	21.198375
77.081707	2673.604180	21.203392
77.059409	2680.552194	21.208410
77.043121	2678.394938	21.213427
77.406902	2665.038742	21.218445
77.346537	2672.095862	21.223463
77.174603	2673.041984	21.228480
77.514423	2667.818598	21.233498
77.247039	2676.199463	21.238515
77.315653	2666.664206	21.243533
77.518737	2671.413261	21.248551
77.667735	2671.144893	21.253568
77.892668	2685.660987	21.258586
77.860774	2701.025844	21.263603
77.712279	2699.527562	21.268621
77.651762	2699.464862	21.273639
77.691996	2702.308918	21.278656
77.784392	2705.736141	21.283674
77.821802	2707.958486	21.288691
77.982868	2724.927834	21.293709
78.424393	2727.292594	21.298727
78.452794	2724.793919	21.303744
78.954461	2723.003172	21.308762
78.662160	2732.386177	21.313779
79.148483	2721.999287	21.318797
78.748210	2723.492301	21.323815
78.876476	2722.793062	21.328832
79.178283	2716.377015	21.333850
79.281480	2708.339316	21.338867
79.238286	2713.877246	21.343885
79.044922	2722.790627	21.348903
79.218981	2713.951925	21.353920
79.372879	2716.062093	21.358938
79.249697	2723.977946	21.363955
79.447416	2705.013339	21.368973
79.008772	2707.074856	21.373991
79.489674	2725.725181	21.379008
79.750418	2738.657007	21.384026
79.516020	2742.374683	21.389043
79.576171	2738.314354	21.394061
79.802252	2743.747213	21.399079
79.756821	2756.347979	21.404096
79.944615	2742.622570	21.409114
79.977057	2754.823931	21.414131
80.414600	2759.557647	21.419149
80.521318	2774.359325	21.424167
80.247666	2768.955302	21.429184
80.737638	2755.497883	21.434202
80.472549	2766.517322	21.439219
80.772906	2758.629059	21.444237
80.613091	2765.703658	21.449255
80.828732	2766.133345	21.454272
81.057081	2759.559100	21.459290
80.883391	2763.156981	21.464307
81.204987	2745.138455	21.469325
80.901591	2770.100165	21.474343
80.935292	2755.895924	21.479360
81.315071	2756.289209	21.484378
81.165808	2752.274072	21.489395
81.307201	2748.836318	21.494413
81.264742	2760.608373	21.499431
81.149347	2779.997270	21.504448
81.514912	2776.204416	21.509466
81.519689	2776.427048	21.514483
81.853128	2773.539924	21.519501
81.808815	2780.769938	21.524519
81.710973	2788.262549	21.529536
81.811056	2771.472524	21.534554
81.452986	2786.178444	21.539571
81.997928	2798.456991	21.544589
82.102059	2801.257054	21.549607
82.427581	2803.018162	21.554624
82.685537	2814.059619	21.559642
82.666107	2811.761263	21.564659
82.640128	2813.261449	21.569677
82.863168	2811.060499	21.574695
82.656548	2808.204440	21.579712
82.994243	2800.097043	21.584730
82.733178	2805.012194	21.589747
82.717448	2809.357293	21.594765
82.579968	2807.085631	21.599783
83.221945	2820.563952	21.604800
83.122935	2822.475357	21.609818
83.145470	2823.964661	21.614835
83.089300	2834.461593	21.619853
83.464242	2826.268799	21.624871
83.215077	2824.175404	21.629888
83.533742	2816.730955	21.634906
83.623572	2842.426071	21.639923
83.813682	2846.024945	21.644941
84.113655	2848.530286	21.649959
84.309756	2841.827432	21.654976
84.391970	2844.764713	21.659994
84.056919	2850.305980	21.665011
84.222873	2842.732494	21.670029
84.674008	2842.818656	21.675047
84.391643	2846.927848	21.680064
84.555424	2834.072971	21.685082
84.752285	2833.569652	21.690099
84.501992	2841.756752	21.695117
84.565024	2838.234728	21.700135
84.208904	2841.400800	21.705152
85.031738	2840.552243	21.710170
84.587214	2847.818587	21.715187
84.762351	2842.256440	21.720205
84.790144	2848.029293	21.725223
84.836040	2855.772738	21.730240
85.186786	2857.299369	21.735258
85.295997	2863.430500	21.740275
85.245110	2868.371930	21.745293
85.074880	2865.493538	21.750311
85.054561	2871.892310	21.755328
85.677931	2886.633729	21.760346
85.693066	2901.786792	21.765363
85.784010	2895.172261	21.770381
86.136920	2903.223867	21.775399
85.908317	2894.467365	21.780416
86.185278	2896.323538	21.785434
86.164596	2892.246168	21.790451
86.355285	2898.648268	21.795469
86.112578	2899.011050	21.800487
86.462273	2893.561053	21.805504
86.831071	2886.117226	21.810522
86.752868	2880.996614	21.815539
86.318011	2883.405995	21.820557
86.698919	2887.011419	21.825575
86.445076	2889.548459	21.830592
86.752756	2887.734358	21.835610
86.977015	2913.096682	21.840627
86.991511	2907.167636	21.845645
87.172026	2908.162176	21.850663
87.150271	2908.161724	21.855680
87.556124	2910.724914	21.860698
86.891184	2911.402802	21.865715
87.190000	2918.121168	21.870733
87.489593	2911.414363	21.875751
87.720116	2924.837270	21.880768
87.566690	2938.143660	21.885786
87.919395	2933.037683	21.890803
88.055091	2925.993617	21.895821
88.403670	2927.141479	21.900839
87.819047	2933.517008	21.905856
88.081391	2928.126550	21.910874
87.897809	2920.974519	21.915891
87.805628	2923.557360	21.920909
88.169225	2936.248789	21.925927
88.296201	2952.217038	21.930944
88.667567	2943.340439	21.935962
88.761108	2952.394618	21.940979
89.072641	2952.101111	21.945997
89.040879	2945.212739	21.951015
88.934669	2951.900541	21.956032
89.174839	2945.811211	21.961050
89.501230	2942.606621	21.966067
89.420987	2943.024510	21.971085
89.813094	2944.376230	21.976103
89.149532	2940.499694	21.981120
89.363661	2938.341834	21.986138
89.498623	2939.761307	21.991155
89.490137	2933.131154	21.996173
89.470121	2932.944796	22.001191
89.680357	2950.160626	22.006208
90.024405	2955.730491	22.011226
90.166484	2968.417949	22.016243
89.871062	2977.593168	22.021261
90.092082	2971.121465	22.026279
89.978063	2973.715662	22.031296
89.641214	2981.959905	22.036314
90.128859	2976.980268	22.041331
89.916427	2976.786841	22.046349
90.339328	2987.832014	22.051367
90.177817	2993.784563	22.056384
90.677787	2994.634561	22.061402
90.658642	2989.452579	22.066419
90.597829	2988.605718	22.071437
91.063708	3001.910147	22.076455
90.765066	3013.510889	22.081472
91.265744	3019.416048	22.086490
91.340917	3028.129474	22.091507
91.117906	3029.261528	22.096525
91.350054	3026.756265	22.101543
91.233125	3031.307919	22.106560
91.274155	3025.601911	22.111578
91.495885	3030.307997	22.116595
91.749828	3051.133620	22.121613
91.977095	3052.351179	22.126631
91.963802	3054.227707	22.131648
91.881955	3054.624618	22.136666
92.024954	3054.896788	22.141683
92.071706	3052.771110	22.146701
92.498785	3047.697282	22.151719
92.243164	3050.459591	22.156736
92.124562	3053.868633	22.161754
92.811157	3065.968292	22.166771
92.699338	3076.250100	22.171789
92.899960	3071.292609	22.176807
92.849413	3084.288546	22.181824
93.041288	3076.658105	22.186842
92.919136	3081.770647	22.191859
92.828303	3084.756025	22.196877
93.214647	3075.254780	22.201895
92.913824	3074.226737	22.206912
93.233641	3088.348189	22.211930
93.908352	3095.187603	22.216947
93.592068	3102.883539	22.221965
93.473903	3108.078831	22.226983
93.787072	3101.649007	22.232000
93.849928	3102.075543	22.237018
94.072971	3098.674240	22.242035
93.968738	3103.586502	22.247053
94.212946	3096.293010	22.252071
93.901041	3107.152631	22.257088
93.881620	3117.087798	22.262106
94.411315	3119.473175	22.267123
94.306204	3131.840733	22.272141
94.697151	3138.645978	22.277159
94.806767	3129.477502	22.282176
94.634584	3125.864709	22.287194
94.623557	3130.431755	22.292211
94.315150	3131.090546	22.297229
95.181969	3145.774529	22.302247
94.824607	3148.327335	22.307264
94.850360	3154.744840	22.312282
95.075604	3149.235939	22.317299
94.952074	3146.633997	22.322317
95.438746	3155.410085	22.327335
95.962162	3169.768943	22.332352
95.904176	3157.282657	22.337370
95.934152	3165.878308	22.342387
96.204384	3166.936430	22.347405
96.062324	3149.531728	22.352423
96.064821	3161.784614	22.357440
95.909331	3167.177804	22.362458
96.117023	3163.764776	22.367475
96.208046	3172.968158	22.372493
96.353952	3163.942537	22.377511
96.583763	3157.643182	22.382528
96.293104	3168.154940	22.387546
96.449017	3153.767213	22.392563
96.348387	3171.592137	22.397581
96.699269	3179.085752	22.402599
97.134435	3186.282763	22.407616
97.048277	3189.530920	22.412634
97.324036	3177.317822	22.417651
97.437165	3188.555708	22.422669
97.257011	3183.539345	22.427687
97.507605	3181.279672	22.432704
97.081294	3181.711070	22.437722
97.534487	3194.673965	22.442739
97.592440	3212.332064	22.447757
97.768728	3212.403071	22.452775
97.648662	3210.672880	22.457792
97.843045	3223.754947	22.462810
97.960923	3202.070640	22.467827
98.054303	3221.179842	22.472845
98.260908	3236.570155	22.477863
98.553316	3238.338174	22.482880
98.511079	3237.515079	22.487898
98.190962	3237.525240	22.492915
98.290711	3232.284095	22.497933
98.775136	3227.333992	22.502951
98.985869	3245.046424	22.507968
98.784693	3266.979290	22.512986
99.358555	3250.253169	22.518003
99.236499	3273.587699	22.523021
99.554088	3270.282188	22.528039
99.553610	3266.217222	22.533056
99.404132	3260.045171	22.538074
99.649554	3255.827726	22.543091
99.819425	3264.400338	22.548109
99.950947	3260.024075	22.553127
99.693218	3259.832360	22.558144
99.519858	3260.443662	22.563162
100.143828	3262.132064	22.568179
100.412587	3271.562016	22.573197
99.896683	3281.542650	22.578215
100.295300	3290.229035	22.583232
100.220389	3280.109025	22.588250
100.177831	3285.897990	22.593267
100.081627	3283.536292	22.598285
100.182480	3282.750943	22.603303
100.602280	3310.798059	22.608320
100.441495	3316.855238	22.613338
100.838484	3304.734396	22.618355
100.988447	3314.071625	22.623373
100.626151	3314.274932	22.628391
101.112287	3320.221079	22.633408
101.179492	3337.340617	22.638426
101.226127	3334.172692	22.643443
101.255951	3341.775014	22.648461
101.287702	3358.709091	22.653479
101.958956	3348.798044	22.658496
101.731725	3383.248253	22.663514
102.149176	3375.659555	22.668531
102.104744	3370.809476	22.673549
102.111892	3378.466562	22.678567
102.390017	3379.837290	22.683584
102.294269	3373.108371	22.688602
102.487245	3369.956430	22.693619
102.361350	3363.575275	22.698637
102.543227	3363.763380	22.703655
102.906956	3368.968439	22.708672
102.796309	3392.163686	22.713690
103.088891	3392.458417	22.718707
103.144325	3395.561332	22.723725
103.148065	3396.131810	22.728743
103.235682	3378.649304	22.733760
103.308607	3393.229678	22.738778
103.545392	3389.859154	22.743795
103.500787	3385.271032	22.748813
103.627318	3397.038676	22.753831
104.086382	3398.689680	22.758848
103.872241	3412.076976	22.763866
103.820273	3423.545885	22.768883
104.041694	3422.627245	22.773901
103.848567	3436.027730	22.778919
104.064141	3419.467104	22.783936
104.149924	3413.340062	22.788954
104.317723	3442.213422	22.793971
104.375733	3441.414445	22.798989
104.714552	3439.040768	22.804007
104.948395	3438.906737	22.809024
105.046010	3452.833509	22.814042
104.989234	3439.733247	22.819059
105.228611	3438.565540	22.824077
105.266195	3449.112463	22.829095
105.311696	3441.539786	22.834112
105.571667	3450.824163	22.839130
105.668104	3451.834511	22.844147
105.599566	3460.229733	22.849165
105.522601	3460.566881	22.854183
106.165507	3472.813864	22.859200
105.621321	3470.480314	22.864218
105.978836	3464.286318	22.869235
106.088947	3473.983973	22.874253
106.090006	3472.489290	22.879271
106.258448	3466.089468	22.884288
106.260292	3474.431785	22.889306
106.356030	3470.377376	22.894323
106.370142	3490.760481	22.899341
106.526242	3489.584026	22.904359
106.716966	3489.853314	22.909376
106.919133	3499.738460	22.914394
106.539346	3487.214325	22.919411
106.869955	3499.739246	22.924429
106.848021	3520.831356	22.929447
106.968298	3512.676436	22.934464
106.928193	3531.896218	22.939482
107.423401	3524.133792	22.944499
107.669490	3548.332728	22.949517
107.636832	3555.044472	22.954535
108.094730	3547.458675	22.959552
107.724965	3549.147482	22.964570
107.818155	3551.405111	22.969587
108.123528	3549.489043	22.974605
108.166378	3550.834381	22.979623
108.515106	3566.541401	22.984640
108.597801	3576.124719	22.989658
108.714050	3565.498921	22.994675
108.827453	3572.660912	22.999693
108.681894	3578.911633	23.004711
109.377569	3566.363017	23.009728
109.273342	3566.346613	23.014746
109.051054	3565.110932	23.019763
109.246416	3563.258816	23.024781
109.240731	3568.308117	23.029799
109.651706	3558.314943	23.034816
109.542244	3561.330134	23.039834
109.754899	3578.609250	23.044851
109.799061	3585.318983	23.049869
109.830595	3584.207222	23.054887
110.056438	3581.507009	23.059904
110.163504	3586.020754	23.064922
110.116613	3584.893182	23.069939
110.048762	3579.991706	23.074957
110.228865	3598.812265	23.079975
110.513725	3603.482513	23.084992
110.639618	3613.776346	23.090010
110.790556	3602.050041	23.095027
110.952824	3617.265336	23.100045
110.455698	3617.108645	23.105063
110.978561	3616.473082	23.110080
111.272016	3630.174502	23.115098
111.272737	3642.670348	23.120115
111.556379	3644.288003	23.125133
111.475184	3644.902714	23.130151
111.426430	3636.795131	23.135168
111.191382	3643.860912	23.140186
111.325594	3632.974194	23.145203
111.788250	3648.829108	23.150221
111.670151	3666.152422	23.155239
111.839616	3664.338247	23.160256
112.142112	3668.020877	23.165274
111.977523	3667.568881	23.170291
112.347013	3676.338018	23.175309
112.598315	3691.428281	23.180327
112.680612	3693.043440	23.185344
112.593042	3700.865254	23.190362
113.038937	3690.663478	23.195379
113.012753	3685.114240	23.200397
112.832015	3696.877637	23.205415
113.189227	3698.523683	23.210432
112.941981	3705.688977	23.215450
112.894618	3724.877133	23.220467
113.383440	3718.249124	23.225485
113.673317	3719.002101	23.230503
113.816495	3717.815103	23.235520
113.597666	3732.154444	23.240538
113.674708	3745.408295	23.245555
114.082520	3748.805918	23.250573
113.779231	3752.664622	23.255591
114.123134	3758.553400	23.260608
114.462414	3771.447665	23.265626
114.692350	3785.835845	23.270643
114.666583	3775.979820	23.275661
114.802346	3788.477854	23.280679
115.075565	3774.044854	23.285696
115.103904	3769.199557	23.290714
115.203707	3771.247714	23.295731
115.422159	3765.056105	23.300749
115.141354	3775.275678	23.305767
114.894334	3775.966394	23.310784
115.038309	3791.951732	23.315802
115.461247	3794.491123	23.320819
115.776946	3797.786242	23.325837
115.845782	3808.772089	23.330855
116.396706	3822.013368	23.335872
116.355597	3829.275641	23.340890
116.191909	3831.125122	23.345907
116.675181	3830.473053	23.350925
116.579307	3832.495000	23.355943
116.557101	3829.493696	23.360960
116.740668	3819.800912	23.365978
116.873230	3807.746997	23.370995
116.906644	3818.493078	23.376013
117.017155	3830.049668	23.381031
117.121114	3833.152804	23.386048
117.433838	3839.736446	23.391066
117.495064	3847.551129	23.396083
117.805362	3836.982289	23.401101
117.560532	3851.499734	23.406119
117.729135	3841.202844	23.411136
118.223761	3840.509634	23.416154
117.524123	3844.511015	23.421171
117.738527	3839.556575	23.426189
117.768317	3850.893216	23.431207
117.985142	3876.579343	23.436224
118.221564	3873.798729	23.441242
118.130801	3875.426560	23.446259
118.466483	3882.761710	23.451277
118.523548	3895.656254	23.456295
118.925525	3901.792266	23.461312
118.950219	3901.246361	23.466330
118.847643	3901.165977	23.471347
118.807456	3897.228307	23.476365
119.089570	3906.087033	23.481383
119.387207	3919.608711	23.486400
119.653132	3923.591434	23.491418
119.581025	3910.429478	23.496435
120.267786	3911.473939	23.501453
120.201435	3915.320073	23.506471
120.265926	3903.486961	23.511488
120.576476	3910.926034	23.516506
120.421095	3907.532190	23.521523
120.544647	3903.010697	23.526541
120.536184	3911.042620	23.531559
120.712549	3900.017618	23.536576
120.695714	3906.031632	23.541594
121.042144	3926.497648	23.546611
121.104343	3930.390935	23.551629
121.028456	3931.531058	23.556647
121.056879	3925.335074	23.561664
121.171198	3923.774299	23.566682
121.056864	3937.832874	23.571699
121.258771	3951.822940	23.576717
121.448644	3968.117372	23.581735
121.744883	3967.837305	23.586752
121.871615	3965.850559	23.591770
121.972861	3966.944345	23.596787
122.147228	3973.653159	23.601805
121.846234	3994.836864	23.606823
122.215296	3992.046089	23.611840
122.304543	3986.814216	23.616858
122.426083	3985.342745	23.621875
122.982992	4010.389630	23.626893
122.795273	4014.329085	23.631911
122.917272	4015.838835	23.636928
123.189426	4014.071959	23.641946
123.089209	4010.412856	23.646963
123.129867	4017.537109	23.651981
123.352745	4023.040185	23.656999
123.532808	4040.724651	23.662016
123.683811	4041.176490	23.667034
123.761591	4047.194353	23.672051
123.711004	4043.082885	23.677069
124.160452	4031.231546	23.682087
124.183687	4041.474403	23.687104
124.296236	4056.078225	23.692122
124.348509	4075.013391	23.697139
124.754903	4068.357467	23.702157
124.702780	4059.219709	23.707175
124.549557	4072.154235	23.712192
125.008747	4073.729788	23.717210
124.903938	4064.773486	23.722227
124.559651	4062.094880	23.727245
124.582230	4079.458391	23.732263
124.764488	4088.920762	23.737280
125.303076	4098.854929	23.742298
125.285827	4118.974097	23.747315
125.725827	4121.445537	23.752333
126.045025	4115.801728	23.757351
125.596785	4122.358960	23.762368
126.105871	4130.437480	23.767386
126.342129	4147.532583	23.772403
126.285967	4150.640868	23.777421
126.211982	4143.993078	23.782439
126.572237	4145.987169	23.787456
126.818685	4131.714627	23.792474
126.543644	4144.194306	23.797491
126.917292	4156.531220	23.802509
127.377415	4168.957403	23.807527
127.229977	4178.024027	23.812544
127.730509	4162.313096	23.817562
127.752388	4164.807955	23.822579
127.704590	4165.045284	23.827597
128.013481	4166.447371	23.832615
127.896530	4162.405449	23.837632
127.980167	4152.201340	23.842650
128.099625	4171.048041	23.847667
128.066345	4186.047323	23.852685
128.276899	4193.080066	23.857703
128.257509	4194.387405	23.862720
128.870547	4184.668374	23.867738
128.871826	4197.545334	23.872755
128.672892	4198.860065	23.877773
128.973498	4210.367763	23.882791
129.167492	4214.311693	23.887808
129.694440	4216.177737	23.892826
129.488900	4216.470901	23.897843
129.699959	4221.516543	23.902861
129.713625	4225.428661	23.907879
129.705141	4226.140355	23.912896
129.860887	4234.121098	23.917914
129.853300	4244.501166	23.922931
129.992496	4243.247112	23.927949
130.471489	4240.580356	23.932967
130.356711	4251.621775	23.937984
130.669663	4228.500699	23.943002
130.304063	4248.288571	23.948019
130.574816	4267.047551	23.953037
130.989548	4267.395199	23.958055
130.703650	4270.577903	23.963072
131.219854	4262.999751	23.968090
131.048990	4273.243829	23.973107
131.177175	4281.322602	23.978125
131.520849	4290.079710	23.983143
131.436153	4302.106745	23.988160
131.489938	4289.346011	23.993178
131.651251	4298.697795	23.998195
131.800800	4319.747192	24.003213
132.237346	4320.134628	24.008231
132.095386	4329.470288	24.013248
132.323150	4319.015742	24.018266
132.499328	4324.226670	24.023283
132.358299	4334.603695	24.028301
132.579345	4349.032394	24.033319
132.673661	4349.612066	24.038336
133.068137	4346.348337	24.043354
133.178056	4349.021128	24.048371
133.538170	4365.962221	24.053389
134.065693	4385.366359	24.058407
133.513930	4386.982014	24.063424
133.765919	4379.038456	24.068442
133.552625	4383.718385	24.073459
134.139501	4380.589949	24.078477
134.201837	4373.257178	24.083495
134.110809	4381.395349	24.088512
134.268862	4384.663825	24.093530
134.447408	4399.770357	24.098547
134.325465	4411.860846	24.103565
134.406682	4394.301058	24.108583
134.526815	4419.486734	24.113600
134.696159	4417.901401	24.118618
135.026191	4422.834532	24.123635
135.097041	4433.237624	24.128653
135.642192	4441.873018	24.133671
135.459939	4459.559915	24.138688
135.514793	4446.407911	24.143706
135.528699	4465.887765	24.148723
135.344089	4468.766447	24.153741
135.990022	4472.979785	24.158759
136.098790	4499.457510	24.163776
136.154938	4490.471348	24.168794
136.228805	4501.205972	24.173811
136.435616	4510.254071	24.178829
136.661380	4512.644105	24.183847
136.566140	4521.035539	24.188864
137.029503	4526.156693	24.193882
137.215116	4530.562235	24.198899
137.184192	4537.088503	24.203917
137.279475	4538.657633	24.208935
137.268866	4535.236623	24.213952
137.648253	4554.857338	24.218970
137.957943	4569.791310	24.223987
138.127518	4569.087761	24.229005
138.286777	4555.830906	24.234023
138.295002	4560.635256	24.239040
138.284708	4567.765542	24.244058
138.332312	4564.373789	24.249075
138.618543	4590.344310	24.254093
138.845302	4582.654821	24.259111
139.029214	4589.642446	24.264128
139.320214	4597.361104	24.269146
139.331978	4587.001384	24.274163
139.308310	4593.561919	24.279181
139.545119	4591.478872	24.284199
139.109610	4597.057259	24.289216
139.348923	4604.661446	24.294234
139.607440	4613.804415	24.299251
139.533077	4626.098316	24.304269
139.809635	4631.192656	24.309287
140.019067	4647.308517	24.314304
139.998660	4651.378793	24.319322
140.411939	4652.747764	24.324339
140.345580	4665.168646	24.329357
140.834555	4671.945614	24.334375
140.826168	4682.312745	24.339392
141.034139	4673.683790	24.344410
141.428883	4674.955026	24.349427
141.258425	4699.269491	24.354445
141.635193	4693.466032	24.359463
141.612738	4687.158267	24.364480
141.752688	4705.613779	24.369498
141.987885	4699.854132	24.374515
142.318943	4694.683354	24.379533
142.551467	4704.004377	24.384551
142.502268	4717.383864	24.389568
142.453368	4718.057187	24.394586
142.913239	4718.697369	24.399603
142.978014	4721.154802	24.404621
143.248316	4708.776895	24.409639
143.136837	4712.353528	24.414656
143.388070	4717.838973	24.419674
143.314285	4728.028554	24.424691
143.367197	4736.206901	24.429709
143.655436	4733.417079	24.434727
143.760367	4746.111221	24.439744
143.573387	4741.532789	24.444762
144.349496	4737.301889	24.449779
144.420486	4753.627168	24.454797
144.437467	4770.901925	24.459815
144.588403	4773.942706	24.464832
144.670535	4770.937157	24.469850
145.061174	4760.062996	24.474867
144.642750	4778.942755	24.479885
144.762180	4770.896619	24.484903
144.875865	4785.034497	24.489920
144.990385	4804.036199	24.494938
145.487461	4798.564367	24.499955
145.644230	4806.250261	24.504973
145.614665	4821.743626	24.509991
145.719234	4821.508270	24.515008
145.677169	4820.401858	24.520026
145.792616	4822.068498	24.525043
146.103663	4837.427326	24.530061
146.520517	4845.665701	24.535079
146.556881	4850.729193	24.540096
146.253313	4848.769251	24.545114
146.952904	4852.651614	24.550131
147.009325	4862.866939	24.555149
147.075215	4877.119514	24.560167
147.392902	4878.746831	24.565184
147.574927	4878.806711	24.570202
147.628288	4870.374575	24.575219
147.482177	4873.720770	24.580237
147.584187	4889.619599	24.585255
147.774966	4904.605129	24.590272
147.539459	4917.168836	24.595290
147.992754	4916.770885	24.600307
147.893710	4927.236819	24.605325
148.285327	4939.406332	24.610343
148.722738	4949.597153	24.615360
148.666372	4952.999068	24.620378
148.990052	4967.612614	24.625395
148.796861	4968.755787	24.630413
148.990136	4966.480602	24.635431
149.737687	4992.086420	24.640448
149.097642	5007.256454	24.645466
149.727245	4998.325649	24.650483
149.874479	5000.857302	24.655501
150.360280	5014.949439	24.660519
150.781770	5018.635471	24.665536
150.811885	5009.883638	24.670554
151.168037	5002.268487	24.675571
151.001145	5017.484233	24.680589
151.386357	5003.831435	24.685607
151.370109	5010.176997	24.690624
151.041513	5017.932529	24.695642
151.430871	5004.125668	24.700659
151.460642	4992.218548	24.705677
151.564480	4996.775727	24.710695
151.807721	4994.786000	24.715712
151.912164	5025.389899	24.720730
152.274726	5014.192772	24.725747
152.114568	5025.333261	24.730765
152.330984	5032.123966	24.735783
152.403220	5018.382605	24.740800
152.507179	5041.140314	24.745818
152.882330	5042.738034	24.750835
153.061763	5055.315936	24.755853
153.214611	5055.476445	24.760871
153.452920	5057.287149	24.765888
153.156335	5047.172941	24.770906
153.427532	5062.885286	24.775923
153.019578	5074.441357	24.780941
153.365771	5081.922549	24.785959
153.651172	5096.949828	24.790976
153.695795	5101.760352	24.795994
154.222964	5102.219113	24.801011
154.078411	5116.674613	24.806029
154.056600	5124.095717	24.811047
154.670380	5130.595756	24.816064
154.646651	5137.245438	24.821082
154.728792	5134.235095	24.826099
154.915882	5146.246230	24.831117
155.525923	5165.772773	24.836135
155.726351	5157.576627	24.841152
155.634051	5161.493305	24.846170
155.917403	5163.699623	24.851187
156.150894	5163.014176	24.856205
155.905537	5162.290228	24.861223
156.365381	5165.495026	24.866240
156.513734	5187.178353	24.871258
156.726698	5175.924716	24.876275
156.618831	5176.463499	24.881293
156.697600	5182.240159	24.886311
157.346074	5187.669522	24.891328
157.391128	5216.341751	24.896346
157.561933	5205.234844	24.901363
157.393228	5212.156270	24.906381
157.659616	5216.784360	24.911399
157.488504	5211.419710	24.916416
157.920985	5221.774353	24.921434
158.124389	5217.655883	24.926451
158.228017	5237.245177	24.931469
158.377679	5227.533275	24.936487
158.731072	5221.677484	24.941504
158.389914	5237.407415	24.946522
158.718080	5247.712628	24.951539
158.918557	5250.481282	24.956557
159.038301	5257.910564	24.961575
159.058490	5260.524669	24.966592
159.410923	5290.445279	24.971610
159.517245	5287.570293	24.976627
159.591396	5288.091070	24.981645
159.678034	5310.139217	24.986663
160.227292	5317.614112	24.991680
160.034039	5323.728425	24.996698
160.316102	5332.805156	25.001715
160.350562	5333.407786	25.006733
160.628590	5347.372104	25.011751
160.798029	5350.598075	25.016768
160.983645	5364.857207	25.021786
161.503238	5376.840687	25.026803
161.595973	5374.945712	25.031821
161.452374	5373.235533	25.036839
161.740456	5381.777169	25.041856
161.764029	5389.069233	25.046874
162.214802	5393.793851	25.051891
162.444252	5389.442252	25.056909
162.515296	5395.899933	25.061927
162.650003	5403.951539	25.066944
162.446122	5406.552623	25.071962
162.752990	5391.537602	25.076979
162.875977	5397.735259	25.081997
162.747980	5415.284060	25.087015
163.426519	5416.879863	25.092032
163.417344	5434.569440	25.097050
163.340986	5429.031475	25.102067
163.891452	5417.540540	25.107085
163.898088	5438.239076	25.112103
163.984188	5448.849719	25.117120
164.017232	5454.050047	25.122138
164.175540	5452.085604	25.127155
164.578393	5453.434292	25.132173
164.573704	5477.810933	25.137191
164.995835	5476.919175	25.142208
165.041718	5483.503632	25.147226
165.137595	5480.528003	25.152243
165.414339	5487.874151	25.157261
165.610876	5497.855168	25.162279
165.744152	5499.500162	25.167296
165.551942	5512.601868	25.172314
166.028304	5500.638863	25.177331
166.092233	5521.556524	25.182349
166.115681	5538.846100	25.187367
166.456876	5526.988803	25.192384
166.709610	5541.301128	25.197402
166.896016	5551.926533	25.202419
167.109460	5553.453332	25.207437
167.197413	5557.583678	25.212455
167.542307	5559.737763	25.217472
167.662125	5558.488264	25.222490
167.556215	5552.370443	25.227507
167.968973	5581.628278	25.232525
167.855174	5589.914713	25.237543
168.145944	5579.697043	25.242560
168.359982	5584.004755	25.247578
167.964080	5611.549911	25.252595
168.099779	5607.075523	25.257613
168.409582	5624.403718	25.262631
168.865197	5629.181925	25.267648
168.924236	5645.253633	25.272666
169.153335	5650.032562	25.277683
169.788051	5653.114396	25.282701
169.583015	5669.706557	25.287719
169.724539	5666.215397	25.292736
169.957954	5665.683351	25.297754
170.133445	5685.497797	25.302771
170.311265	5690.753009	25.307789
170.298734	5700.044510	25.312807
170.386449	5695.958516	25.317824
170.384146	5713.041563	25.322842
170.621007	5719.547685	25.327859
171.247654	5725.059405	25.332877
171.602712	5752.280538	25.337895
171.675515	5747.499878	25.342912
171.861765	5747.340385	25.347930
171.970766	5755.132733	25.352947
172.161220	5751.055517	25.357965
172.030233	5752.281661	25.362983
172.246797	5747.869075	25.368000
172.465501	5772.084710	25.373018
172.386857	5777.356457	25.378035
173.049593	5766.200588	25.383053
172.755377	5772.038525	25.388071
173.013621	5789.054156	25.393088
173.158364	5807.658978	25.398106
172.957571	5812.911665	25.403123
173.308915	5816.349471	25.408141
173.288661	5833.663669	25.413159
173.886191	5833.055466	25.418176
174.156836	5838.641300	25.423194
174.494724	5851.439290	25.428211
174.949211	5850.605291	25.433229
174.601144	5863.255406	25.438247
174.806547	5862.275455	25.443264
175.106664	5868.563864	25.448282
175.224368	5885.237763	25.453299
175.344646	5884.527068	25.458317
175.772977	5886.553825	25.463335
175.832337	5881.306379	25.468352
175.879054	5900.117334	25.473370
176.193728	5906.418386	25.478387
176.512583	5913.739154	25.483405
176.360547	5911.303323	25.488423
176.687728	5909.688736	25.493440
176.680424	5931.898336	25.498458
176.955005	5943.786819	25.503475
177.214508	5931.940652	25.508493
177.312682	5935.304778	25.513511
178.064157	5946.638898	25.518528
178.311151	5962.330892	25.523546
178.249433	5959.113595	25.528563
178.294252	5948.930953	25.533581
178.439411	5954.656422	25.538599
178.565697	5952.202956	25.543616
179.003042	5944.264411	25.548634
178.826525	5945.819600	25.553651
179.124017	5956.098736	25.558669
178.940090	5975.009500	25.563687
179.433554	5975.209333	25.568704
179.426227	5981.517702	25.573722
179.107673	5994.790244	25.578739
179.738765	5999.760880	25.583757
179.598927	6020.515057	25.588775
179.936348	6016.881653	25.593792
180.032656	6027.979644	25.598810
180.189628	6044.003917	25.603827
180.091351	6054.498850	25.608845
180.418654	6076.004690	25.613863
180.683206	6083.487614	25.618880
180.976551	6085.346320	25.623898
180.639843	6102.828512	25.628915
181.303628	6099.953387	25.633933
181.326012	6109.053910	25.638951
181.604353	6125.068360	25.643968
181.967492	6124.156078	25.648986
181.838352	6129.924564	25.654003
182.495433	6144.571095	25.659021
182.718174	6146.762842	25.664039
182.836696	6156.078579	25.669056
183.314186	6158.438194	25.674074
183.280889	6153.834814	25.679092
183.559571	6157.078949	25.684109
183.702350	6175.002449	25.689127
183.228767	6179.201260	25.694144
183.911929	6177.635310	25.699162
183.846122	6186.737354	25.704180
184.456463	6194.988917	25.709197
184.315514	6208.838334	25.714215
184.650537	6195.371821	25.719232
184.551442	6212.005130	25.724250
184.545475	6237.093655	25.729268
185.012590	6235.567653	25.734285
185.291568	6239.596927	25.739303
185.409335	6257.415945	25.744320
185.797029	6264.672415	25.749338
185.877330	6268.156692	25.754356
186.156594	6272.980539	25.759373
186.282605	6294.247366	25.764391
186.966353	6289.365975	25.769408
186.796885	6278.998557	25.774426
186.974667	6283.120292	25.779444
187.254365	6278.710073	25.784461
187.613120	6294.270524	25.789479
187.369806	6307.522695	25.794496
187.433683	6305.245912	25.799514
187.730760	6303.926392	25.804532
187.756281	6302.145866	25.809549
187.894761	6324.138487	25.814567
188.070868	6333.252402	25.819584
188.514934	6337.245941	25.824602
188.495918	6371.072804	25.829620
188.993563	6374.800544	25.834637
189.094313	6377.952726	25.839655
189.142543	6368.737738	25.844672
189.423069	6382.692416	25.849690
189.465956	6391.379948	25.854708
189.601754	6388.016200	25.859725
189.650264	6415.153689	25.864743
189.931780	6423.933794	25.869760
190.381615	6426.552772	25.874778
190.307574	6437.092890	25.879796
190.409195	6452.413635	25.884813
190.458960	6454.356857	25.889831
191.225399	6465.203572	25.894848
191.433689	6475.827730	25.899866
191.467966	6491.431470	25.904884
191.919002	6479.979175	25.909901
191.985601	6483.388587	25.914919
191.935177	6475.308812	25.919936
192.525283	6490.983642	25.924954
192.360444	6507.918077	25.929972
192.255612	6498.907579	25.934989
192.839943	6508.622898	25.940007
192.540480	6516.214065	25.945024
192.983616	6530.222419	25.950042
193.028024	6532.928873	25.955060
193.554561	6546.850777	25.960077
193.324887	6557.809960	25.965095
193.588865	6564.976945	25.970112
194.031429	6574.954873	25.975130
193.838597	6585.259912	25.980148
194.080369	6596.651417	25.985165
194.377199	6606.762748	25.990183
194.491237	6629.020137	25.995200
194.897218	6628.227666	26.000218
195.070150	6653.201830	26.005236
195.034969	6642.864672	26.010253
195.488990	6656.333266	26.015271
195.649972	6673.668330	26.020288
196.454175	6676.385061	26.025306
196.599820	6678.954239	26.030324
196.781349	6674.967886	26.035341
197.079719	6672.947910	26.040359
196.730983	6693.880314	26.045376
197.037763	6696.281400	26.050394
197.289588	6704.710002	26.055412
197.295670	6698.058517	26.060429
197.754209	6714.500417	26.065447
197.987800	6729.716225	26.070464
198.314664	6722.534445	26.075482
198.328600	6737.085847	26.080500
198.316622	6730.824316	26.085517
198.605265	6744.773323	26.090535
198.619963	6760.621219	26.095552
199.263739	6752.649335	26.100570
199.191468	6764.178370	26.105588
198.994578	6789.203859	26.110605
199.299349	6778.718780	26.115623
199.353202	6795.316556	26.120640
199.798108	6815.261870	26.125658
199.954901	6810.755435	26.130676
200.080761	6835.951414	26.135693
200.664972	6839.772476	26.140711
200.456600	6852.766220	26.145728
200.753099	6853.593852	26.150746
201.037720	6877.324795	26.155764
201.416366	6878.745147	26.160781
201.295040	6882.455263	26.165799
201.890357	6905.013988	26.170816
202.392643	6894.431248	26.175834
202.278233	6908.503678	26.180852
202.336595	6909.690285	26.185869
202.590998	6900.741857	26.190887
202.556258	6905.672625	26.195904
202.662384	6912.957788	26.200922
202.984736	6924.889804	26.205940
203.327365	6930.621936	26.210957
203.637663	6938.752603	26.215975
203.481338	6964.834858	26.220992
203.884392	6956.259234	26.226010
204.163109	6952.162898	26.231028
204.270024	6975.419580	26.236045
204.511280	6965.554251	26.241063
204.497509	6986.529649	26.246080
204.551702	6976.868801	26.251098
204.819158	6993.516143	26.256116
205.122037	7009.213719	26.261133
205.459044	7019.794144	26.266151
205.446164	7030.838702	26.271168
205.693461	7031.439727	26.276186
205.955477	7056.333493	26.281204
205.878632	7060.074327	26.286221
206.284583	7058.156740	26.291239
206.459032	7086.987425	26.296256
206.598429	7092.910954	26.301274
207.347198	7097.572888	26.306292
207.387721	7117.207785	26.311309
207.481401	7126.190564	26.316327
207.431990	7139.861817	26.321344
208.007607	7146.947144	26.326362
208.108572	7139.988435	26.331380
208.409493	7151.307996	26.336397
208.700107	7163.532443	26.341415
209.170688	7176.507131	26.346432
209.344571	7179.226893	26.351450
209.220659	7172.129354	26.356468
209.877965	7190.330044	26.361485
210.089493	7196.095771	26.366503
210.335674	7197.176139	26.371520
210.621722	7196.706465	26.376538
210.813289	7184.898457	26.381556
210.598642	7184.078235	26.386573
211.080818	7184.399489	26.391591
211.518930	7180.370521	26.396608
211.435618	7201.262108	26.401626
211.800158	7213.067253	26.406644
212.214895	7203.995520	26.411661
212.217785	7200.954121	26.416679
212.208706	7205.011492	26.421696
212.364732	7213.949766	26.426714
212.506666	7206.229173	26.431732
212.346856	7227.769509	26.436749
212.509350	7225.682216	26.441767
212.526467	7220.702246	26.446784
212.588339	7248.457553	26.451802
213.068692	7273.622152	26.456820
213.162164	7268.212992	26.461837
213.613413	7285.978510	26.466855
213.523433	7309.615658	26.471872
213.595187	7313.815958	26.476890
214.272687	7324.751454	26.481908
214.303150	7337.562773	26.486925
214.609592	7357.706354	26.491943
214.563827	7358.492594	26.496960
214.834540	7366.558211	26.501978
215.184738	7392.751655	26.506996
215.545721	7407.511178	26.512013
215.966085	7394.836450	26.517031
215.801673	7419.663482	26.522048
216.180723	7424.216879	26.527066
216.301138	7425.809853	26.532084
216.230889	7441.620879	26.537101
216.818575	7456.229434	26.542119
217.146943	7470.138175	26.547136
217.184695	7464.548993	26.552154
217.813148	7479.933158	26.557172
217.761342	7493.549255	26.562189
218.228363	7503.384652	26.567207
218.314327	7500.772920	26.572224
218.516163	7507.756719	26.577242
219.471948	7507.871868	26.582260
219.164014	7528.204899	26.587277
219.708887	7509.603648	26.592295
219.717654	7514.825883	26.597312
219.870721	7506.189089	26.602330
220.427367	7532.293218	26.607348
220.072982	7537.167362	26.612365
220.536546	7538.765440	26.617383
220.367644	7549.541777	26.622400
220.130892	7551.534757	26.627418
220.608012	7562.022423	26.632436
220.733366	7574.532420	26.637453
221.283915	7600.069562	26.642471
221.127195	7607.101917	26.647488
221.414944	7622.485471	26.652506
221.877503	7644.006656	26.657524
221.792117	7652.092220	26.662541
222.247486	7657.532066	26.667559
222.629126	7661.870324	26.672576
222.805051	7684.824421	26.677594
223.361568	7686.617778	26.682612
223.394053	7692.690777	26.687629
223.371590	7704.764161	26.692647
223.330629	7715.433671	26.697664
223.479129	7727.213872	26.702682
224.307701	7744.775013	26.707700
224.211939	7757.542299	26.712717
224.797729	7754.234757	26.717735
224.857073	7763.758435	26.722752
224.829156	7770.605887	26.727770
225.340291	7785.991766	26.732788
225.366150	7787.388986	26.737805
225.448919	7801.887970	26.742823
225.893697	7803.774691	26.747840
225.812913	7819.598026	26.752858
226.691082	7828.255525	26.757876
226.802237	7838.988997	26.762893
226.921784	7832.102538	26.767911
227.147686	7833.299491	26.772928
226.918516	7848.311691	26.777946
227.548496	7847.965780	26.782964
227.600345	7862.716816	26.787981
227.959596	7870.344495	26.792999
228.001279	7894.366798	26.798016
228.105809	7885.707623	26.803034
228.445545	7904.509820	26.808052
228.387942	7918.320003	26.813069
228.793057	7922.679775	26.818087
229.055756	7939.255766	26.823104
228.746098	7953.583771	26.828122
229.410417	7962.539031	26.833140
229.959861	7991.036301	26.838157
230.363795	7999.645186	26.843175
230.666339	8003.682996	26.848192
230.595243	8017.087842	26.853210
231.043529	8007.553912	26.858228
231.301516	8032.502680	26.863245
231.567962	8027.466955	26.868263
231.615658	8031.343184	26.873280
232.015985	8052.785186	26.878298
232.169043	8053.995344	26.883316
232.573202	8061.047866	26.888333
232.558033	8054.710749	26.893351
232.896222	8082.006539	26.898368
233.051372	8086.181174	26.903386
233.427667	8086.402884	26.908404
233.602849	8098.242074	26.913421
233.808627	8101.742976	26.918439
234.286398	8112.548029	26.923456
233.809930	8122.065296	26.928474
234.224606	8121.774950	26.933492
234.600864	8142.906184	26.938509
234.637433	8148.928754	26.943527
235.166968	8170.833450	26.948544
235.242507	8175.450418	26.953562
235.648492	8185.883776	26.958580
235.334004	8197.694884	26.963597
235.750877	8205.122347	26.968615
235.896736	8227.056818	26.973632
235.919076	8237.469540	26.978650
236.336594	8254.959124	26.983668
236.871564	8263.735331	26.988685
237.124922	8269.962986	26.993703
237.437323	8288.522957	26.998720
237.378768	8298.863639	27.003738
237.788613	8294.874294	27.008756
238.044364	8313.421296	27.013773
238.162044	8321.643237	27.018791
238.465837	8318.910083	27.023808
238.512697	8328.963304	27.028826
239.302879	8339.839894	27.033844
239.211899	8350.253450	27.038861
239.298132	8353.387126	27.043879
239.705008	8372.300388	27.048896
239.746890	8378.860806	27.053914
239.950958	8387.419162	27.058932
239.773970	8407.957554	27.063949
240.421883	8418.554730	27.068967
240.896442	8419.548427	27.073984
241.115254	8438.884396	27.079002
241.073970	8442.678134	27.084020
241.347465	8456.427377	27.089037
241.995215	8464.832427	27.094055
242.206848	8486.462509	27.099072
242.406032	8499.975778	27.104090
242.730821	8485.068094	27.109108
242.895394	8508.096091	27.114125
243.119790	8516.525382	27.119143
243.513752	8512.099444	27.124160
243.525188	8542.714432	27.129178
243.893282	8538.238317	27.134196
243.969219	8542.258894	27.139213
244.144416	8560.231259	27.144231
244.274200	8563.612193	27.149248
244.793547	8587.524846	27.154266
244.953007	8598.682369	27.159284
245.005124	8600.774217	27.164301
245.452323	8616.266365	27.169319
245.803043	8630.763573	27.174336
245.536454	8634.966251	27.179354
246.618411	8652.719425	27.184372
246.798273	8661.175570	27.189389
246.459739	8656.641316	27.194407
247.071984	8673.501546	27.199424
247.275343	8689.284441	27.204442
247.621947	8684.269555	27.209460
247.920317	8698.372296	27.214477
247.856889	8722.222268	27.219495
248.344436	8704.805838	27.224512
248.448902	8737.969237	27.229530
248.846326	8740.587557	27.234548
248.994135	8751.006604	27.239565
248.729453	8762.124062	27.244583
249.393585	8764.161647	27.249600
249.463547	8785.825765	27.254618
249.858147	8792.727510	27.259636
250.049989	8810.023958	27.264653
250.198676	8827.701072	27.269671
250.575892	8831.509242	27.274688
250.665638	8836.692277	27.279706
251.000969	8862.261972	27.284724
251.690575	8860.064460	27.289741
251.835270	8862.942630	27.294759
251.952688	8866.674193	27.299776
252.204530	8881.376259	27.304794
252.521235	8882.432925	27.309812
253.068420	8894.882297	27.314829
252.699731	8901.670493	27.319847
253.327569	8897.401521	27.324864
253.486020	8910.104874	27.329882
253.392594	8918.076733	27.334900
253.780578	8930.114007	27.339917
254.078071	8946.794167	27.344935
254.724368	8936.647366	27.349952
254.477887	8968.003881	27.354970
254.971878	8976.430589	27.359988
255.287856	8971.240294	27.365005
255.338675	8986.344346	27.370023
255.540353	9010.830027	27.375040
255.598759	9010.758957	27.380058
256.022923	9020.731646	27.385076
256.250406	9036.784115	27.390093
256.368225	9049.727376	27.395111
256.939561	9058.727248	27.400128
257.270040	9072.050533	27.405146
257.425135	9084.939096	27.410164
257.622539	9091.372346	27.415181
257.615210	9112.400074	27.420199
257.943640	9111.658806	27.425216
258.239094	9125.310348	27.430234
258.159497	9150.348249	27.435252
258.830073	9158.642649	27.440269
258.913583	9188.001028	27.445287
259.032688	9191.639550	27.450304
259.513959	9225.498992	27.455322
259.594165	9223.066505	27.460340
260.123455	9233.237402	27.465357
260.082002	9250.771424	27.470375
260.562959	9263.032971	27.475392
260.710583	9282.342040	27.480410
261.065246	9292.156413	27.485428
261.554326	9312.969550	27.490445
261.840968	9330.172013	27.495463
262.315950	9325.738040	27.500480
262.330644	9330.572415	27.505498
262.630821	9355.482446	27.510516
262.802827	9351.345031	27.515533
262.885641	9367.044383	27.520551
263.522385	9382.476428	27.525568
263.659695	9381.844305	27.530586
264.079986	9405.087096	27.535604
264.310625	9409.019901	27.540621
264.629359	9421.767781	27.545639
264.979845	9425.662206	27.550656
265.292667	9444.916036	27.555674
265.379957	9451.382734	27.560692
265.642508	9454.806841	27.565709
265.863049	9448.284799	27.570727
266.071224	9450.685147	27.575744
266.141566	9459.523938	27.580762
266.247235	9478.624335	27.585780
266.804072	9487.579566	27.590797
266.827042	9499.500793	27.595815
266.882266	9517.753907	27.600832
267.287766	9525.396711	27.605850
267.212990	9546.802503	27.610868
267.450130	9564.201200	27.615885
267.832011	9570.831883	27.620903
268.063030	9601.187011	27.625920
268.550170	9616.393695	27.630938
268.805824	9635.186305	27.635956
269.431768	9646.174249	27.640973
269.383490	9664.231571	27.645991
269.375647	9672.545877	27.651008
270.085233	9685.612156	27.656026
270.021242	9696.809269	27.661044
270.712184	9713.595185	27.666061
270.597970	9717.470907	27.671079
270.622348	9748.115022	27.676096
271.507219	9751.992027	27.681114
271.655205	9775.680528	27.686132
272.029540	9783.949320	27.691149
272.056733	9810.329538	27.696167
272.554366	9809.661995	27.701184
273.071576	9823.496415	27.706202
273.034072	9842.402512	27.711220
273.764232	9845.181647	27.716237
273.741396	9861.491311	27.721255
273.618974	9863.079980	27.726272
274.206064	9882.677039	27.731290
274.821229	9894.088681	27.736308
274.919579	9918.156359	27.741325
275.446121	9928.908145	27.746343
275.486164	9929.685955	27.751360
275.667515	9927.363142	27.756378
275.748720	9949.193984	27.761396
276.228307	9951.354022	27.766413
276.446715	9989.801268	27.771431
276.346797	9990.410166	27.776448
277.072344	9995.300242	27.781466
277.395086	10005.704873	27.786484
277.931542	10021.079598	27.791501
278.212528	10029.734843	27.796519
278.579115	10032.599120	27.801536
278.516133	10044.715085	27.806554
278.587262	10064.640154	27.811572
279.174835	10059.004856	27.816589
279.332884	10071.139908	27.821607
279.310065	10093.558076	27.826624
279.559935	10090.477112	27.831642
279.901630	10099.165216	27.836660
280.143033	10128.543553	27.841677
280.211067	10129.850855	27.846695
280.495271	10148.360194	27.851712
280.989223	10166.813301	27.856730
281.251361	10175.820254	27.861748
281.419151	10181.788102	27.866765
281.510603	10201.595613	27.871783
281.772528	10223.194620	27.876800
281.895048	10226.599521	27.881818
282.151000	10253.569287	27.886836
282.750413	10268.051271	27.891853
283.334394	10283.834598	27.896871
283.242237	10295.987681	27.901888
283.712345	10305.191746	27.906906
283.760177	10339.564680	27.911924
284.573948	10339.664375	27.916941
284.655715	10347.158140	27.921959
284.704240	10370.667090	27.926976
285.191006	10379.177596	27.931994
285.402319	10398.955638	27.937012
285.679246	10402.744792	27.942029
286.080411	10435.449537	27.947047
286.550221	10434.080502	27.952064
286.836901	10452.540638	27.957082
286.864714	10469.399665	27.962100
287.395243	10487.681682	27.967117
287.909068	10492.015059	27.972135
288.012881	10500.461942	27.977152
288.075910	10511.812548	27.982170
288.289655	10540.181701	27.987188
288.705380	10536.116865	27.992205
289.121695	10552.015735	27.997223
289.115909	10568.254982	28.002240
289.875702	10574.123902	28.007258
290.071733	10590.077207	28.012276
290.444752	10604.103749	28.017293
290.651350	10613.861933	28.022311
290.679489	10621.641398	28.027328
290.818700	10639.030591	28.032346
291.117444	10658.857210	28.037364
291.357791	10677.602024	28.042381
291.680174	10687.380362	28.047399
291.640965	10708.864378	28.052416
292.153535	10727.394695	28.057434
292.480929	10735.718325	28.062452
292.942498	10759.140010	28.067469
293.426640	10767.992313	28.072487
293.162493	10783.071256	28.077504
293.888208	10805.028441	28.082522
294.182373	10830.577374	28.087540
294.427894	10839.037275	28.092557
294.878780	10852.890701	28.097575
294.753902	10869.212608	28.102592
295.239172	10881.275305	28.107610
295.508544	10886.728295	28.112628
295.710198	10900.309451	28.117645
296.301345	10912.689766	28.122663
296.509989	10935.313899	28.127680
296.689545	10936.981251	28.132698
296.901888	10947.867278	28.137716
297.003030	10965.280231	28.142733
297.575804	10980.968103	28.147751
297.767911	10990.615516	28.152768
298.152703	11013.833414	28.157786
298.464664	11022.250562	28.162804
298.739690	11035.098473	28.167821
299.173525	11034.319466	28.172839
299.315472	11073.343981	28.177856
299.718205	11076.748090	28.182874
300.127039	11097.903111	28.187892
300.509341	11115.088053	28.192909
300.927044	11121.582294	28.197927
300.684606	11149.144658	28.202944
301.392590	11140.364206	28.207962
301.360636	11164.349585	28.212980
301.587410	11182.830793	28.217997
301.990458	11191.902863	28.223015
302.247519	11213.576870	28.228032
302.347053	11226.071614	28.233050
302.669411	11246.973048	28.238068
302.876680	11256.972761	28.243085
303.397902	11289.459151	28.248103
303.472433	11309.162605	28.253120
304.022470	11323.760914	28.258138
304.292035	11347.355389	28.263156
304.820431	11366.526962	28.268173
305.129213	11379.785329	28.273191
304.904075	11404.438574	28.278208
305.441402	11416.217558	28.283226
306.111626	11434.010981	28.288244
306.495461	11458.718947	28.293261
306.819414	11466.176242	28.298279
307.024589	11494.085009	28.303296
307.774444	11496.766497	28.308314
307.849476	11514.488035	28.313332
308.355924	11525.216242	28.318349
308.629367	11523.316485	28.323367
308.741802	11549.404021	28.328384
308.951139	11555.058464	28.333402
309.322730	11562.745895	28.338420
309.403471	11580.409542	28.343437
309.651888	11596.797478	28.348455
310.084272	11621.587498	28.353472
310.353257	11636.263963	28.358490
310.568683	11652.331391	28.363508
310.600651	11672.722881	28.368525
311.338203	11689.169505	28.373543
311.195556	11696.805173	28.378560
311.754583	11703.968942	28.383578
312.203378	11728.446433	28.388596
312.350631	11742.279820	28.393613
313.231673	11746.259903	28.398631
313.027147	11770.340648	28.403648
313.314619	11774.196945	28.408666
313.616497	11794.266183	28.413684
313.409667	11808.338265	28.418701
313.968429	11823.281572	28.423719
313.849009	11849.714705	28.428736
314.453815	11863.614974	28.433754
315.018607	11892.745308	28.438772
315.093491	11907.016955	28.443789
315.524064	11917.400222	28.448807
315.868085	11946.027511	28.453824
316.108071	11967.846206	28.458842
316.549284	11985.429654	28.463860
316.671975	12002.124555	28.468877
317.481751	12027.003056	28.473895
317.736575	12041.071426	28.478912
318.110417	12055.203479	28.483930
317.964627	12079.862491	28.488948
318.040990	12095.578708	28.493965
318.863467	12101.225355	28.498983
319.102338	12140.695638	28.504000
319.746930	12155.713747	28.509018
319.998583	12163.548893	28.514036
320.221598	12181.642728	28.519053
320.689970	12192.458943	28.524071
320.900030	12216.682888	28.529088
320.982244	12222.309440	28.534106
321.584947	12257.857205	28.539124
321.853061	12272.665082	28.544141
322.314846	12292.243557	28.549159
322.316792	12309.041076	28.554176
322.801578	12324.452775	28.559194
323.128434	12336.166466	28.564212
323.324305	12365.942876	28.569229
323.776951	12380.968191	28.574247
324.130034	12397.128203	28.579264
324.575613	12415.502458	28.584282
324.798367	12434.003944	28.589300
325.066400	12455.079817	28.594317
325.592506	12476.626968	28.599335
325.643279	12500.443671	28.604352
325.910147	12513.469859	28.609370
326.580816	12525.846709	28.614388
326.892998	12545.081795	28.619405
326.832161	12560.053360	28.624423
327.317791	12577.893697	28.629440
327.707984	12599.204132	28.634458
327.932611	12611.195444	28.639476
327.981536	12640.266785	28.644493
328.487509	12651.838442	28.649511
328.814763	12674.016732	28.654528
329.429213	12677.096446	28.659546
329.501015	12686.234811	28.664564
329.800910	12711.825571	28.669581
329.994523	12727.856889	28.674599
330.085174	12740.347218	28.679616
330.463934	12755.674133	28.684634
330.974462	12782.449060	28.689652
331.265890	12808.601935	28.694669
331.428857	12810.932508	28.699687
331.910530	12845.842943	28.704704
332.074735	12856.118389	28.709722
332.804360	12882.311154	28.714740
333.076738	12905.422769	28.719757
333.578936	12923.970439	28.724775
334.355849	12942.349397	28.729792
334.331306	12955.100490	28.734810
334.771835	12962.770766	28.739828
334.830758	12977.928103	28.744845
335.506513	13001.079471	28.749863
335.572093	13013.514989	28.754880
335.765902	13035.400829	28.759898
336.231251	13048.431068	28.764916
336.070789	13068.289970	28.769933
336.468453	13093.050948	28.774951
336.838984	13114.740297	28.779968
337.182813	13144.977150	28.784986
337.973907	13160.313731	28.790004
338.369679	13190.405243	28.795021
338.832137	13201.692440	28.800039
338.763803	13215.741389	28.805056
339.113353	13238.546048	28.810074
339.750738	13245.000497	28.815092
339.946392	13272.692689	28.820109
340.609392	13289.438673	28.825127
340.751445	13305.066177	28.830144
340.946180	13330.471077	28.835162
341.211744	13344.296913	28.840180
341.262076	13370.019668	28.845197
341.844212	13384.102848	28.850215
342.320579	13406.248214	28.855232
342.707264	13425.580577	28.860250
343.400544	13441.883874	28.865268
343.142477	13466.009684	28.870285
343.697885	13481.326106	28.875303
344.085320	13503.210688	28.880320
344.395872	13515.163441	28.885338
344.661398	13531.512771	28.890356
344.856824	13550.971216	28.895373
345.752563	13567.392722	28.900391
346.046174	13596.428668	28.905408
346.164487	13603.847385	28.910426
346.656652	13619.265923	28.915444
346.672100	13638.930661	28.920461
347.087643	13664.884980	28.925479
347.605806	13674.059064	28.930496
347.703871	13703.567566	28.935514
348.071280	13707.942938	28.940532
348.298655	13733.010747	28.945549
348.408354	13743.664451	28.950567
348.879565	13750.337861	28.955584
349.053819	13779.791076	28.960602
349.871553	13790.474050	28.965620
349.809192	13813.877719	28.970637
349.823517	13841.382006	28.975655
350.292469	13862.534473	28.980672
350.768461	13890.207120	28.985690
350.949452	13913.139427	28.990708
351.472490	13937.046054	28.995725
351.699605	13957.606890	29.000743
352.074205	13995.295194	29.005760
352.323580	14026.320850	29.010778
353.115052	14038.773466	29.015796
353.134648	14071.796722	29.020813
353.412002	14091.119808	29.025831
354.130607	14121.925058	29.030848
354.523153	14144.709271	29.035866
355.054380	14158.684788	29.040884
355.261641	14193.380624	29.045901
355.597436	14210.092107	29.050919
356.240404	14222.942738	29.055936
356.267263	14248.646217	29.060954
356.914951	14258.032326	29.065972
357.337378	14287.113608	29.070989
357.469535	14299.351041	29.076007
358.046134	14315.799725	29.081024
358.175846	14344.018320	29.086042
358.860835	14352.144786	29.091060
358.863416	14379.032807	29.096077
359.092490	14396.647263	29.101095
359.685176	14430.469365	29.106112
359.799185	14446.884563	29.111130
360.483181	14471.260034	29.116148
360.876104	14500.868321	29.121165
360.715313	14529.776553	29.126183
361.268402	14538.903288	29.131200
361.840662	14569.317140	29.136218
362.496569	14584.708598	29.141236
362.442757	14608.656358	29.146253
362.923984	14623.557632	29.151271
363.579321	14644.731275	29.156288
363.912746	14658.930654	29.161306
364.314286	14675.499039	29.166324
364.521557	14695.474631	29.171341
365.127237	14729.289717	29.176359
365.445418	14733.446329	29.181376
365.513617	14751.759286	29.186394
365.912024	14773.084163	29.191412
366.233329	14793.378626	29.196429
366.230677	14807.329028	29.201447
366.919500	14819.533072	29.206464
366.918171	14842.526435	29.211482
367.393929	14871.879590	29.216500
367.599678	14888.029332	29.221517
368.069033	14907.444280	29.226535
368.590503	14930.153528	29.231552
368.710365	14953.673566	29.236570
369.325369	14972.165522	29.241588
369.366475	14999.613505	29.246605
369.674400	15021.780987	29.251623
370.111082	15035.467144	29.256640
370.434731	15075.553818	29.261658
371.091890	15097.709542	29.266676
371.395498	15117.830924	29.271693
371.545867	15147.921801	29.276711
372.369633	15166.873024	29.281728
372.491649	15193.273775	29.286746
372.763089	15211.802963	29.291764
372.973005	15237.614233	29.296781
373.312574	15268.323586	29.301799
374.542891	15280.247563	29.306816
374.514044	15310.561884	29.311834
375.056665	15334.412679	29.316852
375.435890	15346.788112	29.321869
376.007977	15367.742226	29.326887
376.628164	15388.257308	29.331904
376.943617	15413.778893	29.336922
377.374544	15421.490528	29.341940
377.663451	15435.671649	29.346957
377.511265	15466.245346	29.351975
378.223065	15464.600679	29.356992
378.320099	15500.623838	29.362010
378.619810	15521.764943	29.367028
379.363096	15532.582354	29.372045
379.481262	15564.828433	29.377063
379.956740	15588.538980	29.382080
380.089789	15625.246896	29.387098
380.717204	15642.208494	29.392116
381.092166	15658.612535	29.397133
381.276978	15689.333029	29.402151
381.978510	15710.643481	29.407168
381.738963	15733.609523	29.412186
382.350696	15755.927447	29.417204
382.706308	15780.784719	29.422221
382.972339	15821.050406	29.427239
383.277458	15830.331982	29.432256
383.727942	15864.924360	29.437274
384.305223	15886.660191	29.442292
384.855476	15913.746348	29.447309
384.661084	15948.095390	29.452327
385.254440	15960.216375	29.457344
385.984330	15997.530524	29.462362
386.247944	16021.823924	29.467380
386.628051	16050.104734	29.472397
386.887114	16073.929148	29.477415
387.326334	16085.088661	29.482432
387.874738	16112.541243	29.487450
388.011818	16137.016475	29.492468
388.322230	16153.030325	29.497485
388.702102	16179.221240	29.502503
389.239034	16198.280472	29.507520
389.602823	16232.880410	29.512538
389.774421	16252.945103	29.517556
390.097326	16279.507212	29.522573
390.123670	16303.551319	29.527591
390.617192	16334.365812	29.532608
391.105321	16369.671023	29.537626
391.513946	16398.969019	29.542644
392.426006	16424.317503	29.547661
392.454736	16449.659177	29.552679
393.372440	16464.011183	29.557696
393.425666	16507.493167	29.562714
393.823865	16525.586686	29.567732
394.158425	16545.555429	29.572749
394.514193	16578.825448	29.577767
395.073902	16602.704037	29.582784
395.451185	16621.799079	29.587802
396.161135	16655.033292	29.592820
396.676317	16677.625981	29.597837
396.776262	16710.492432	29.602855
397.217487	16728.490961	29.607872
397.650886	16743.614991	29.612890
397.753872	16775.559182	29.617908
398.476890	16791.470257	29.622925
398.708812	16833.126118	29.627943
399.333522	16846.959900	29.632960
399.328907	16884.761214	29.637978
399.890838	16899.166387	29.642996
400.789665	16926.238843	29.648013
400.871483	16941.141963	29.653031
401.414626	16966.833169	29.658048
401.692128	16983.642890	29.663066
402.402468	17010.201307	29.668084
402.547199	17037.847414	29.673101
402.828992	17050.615888	29.678119
402.975511	17084.147875	29.683136
403.604967	17114.154966	29.688154
404.056225	17132.952472	29.693172
404.634276	17149.981774	29.698189
404.652964	17185.633514	29.703207
405.217316	17202.546567	29.708224
406.032575	17228.580828	29.713242
406.161770	17253.983594	29.718260
406.361230	17279.761777	29.723277
406.654025	17309.030462	29.728295
407.255716	17318.504437	29.733312
407.554484	17364.514199	29.738330
407.585512	17391.295488	29.743348
408.353834	17420.928724	29.748365
408.472479	17459.864050	29.753383
409.126159	17474.087052	29.758400
409.322498	17491.092723	29.763418
409.647815	17505.482830	29.768436
409.872521	17545.824567	29.773453
410.390415	17572.989767	29.778471
410.783315	17599.194901	29.783488
411.423493	17625.296116	29.788506
411.442435	17660.565675	29.793524
412.101512	17686.283896	29.798541
412.322040	17718.227840	29.803559
412.629336	17748.880567	29.808576
413.213233	17781.674347	29.813594
413.411297	17816.954890	29.818612
414.047045	17851.017231	29.823629
414.635982	17868.815619	29.828647
415.231704	17905.812008	29.833664
415.730777	17929.598195	29.838682
415.942757	17958.538098	29.843700
416.619672	17984.282909	29.848717
416.865400	18006.303989	29.853735
417.416805	18034.320318	29.858752
417.846639	18054.951388	29.863770
418.037917	18084.560534	29.868788
418.656778	18103.717930	29.873805
418.733355	18138.863653	29.878823
419.271317	18151.644580	29.883840
420.008817	18187.557889	29.888858
420.340165	18219.871608	29.893876
421.001897	18245.322833	29.898893
421.087972	18279.589449	29.903911
421.393230	18303.538585	29.908928
421.951869	18331.679493	29.913946
421.838749	18366.858320	29.918964
422.767255	18382.361354	29.923981
423.052246	18423.516015	29.928999
423.347763	18458.547657	29.934016
424.037022	18484.072839	29.939034
424.142099	18516.574014	29.944052
425.018716	18549.313334	29.949069
425.485053	18580.999227	29.954087
425.401942	18606.323673	29.959104
426.291131	18627.397262	29.964122
426.598167	18662.183833	29.969140
426.768593	18693.930887	29.974157
427.259283	18729.260776	29.979175
427.658712	18751.796016	29.984192
428.308143	18778.749271	29.989210
428.499986	18821.038319	29.994228
429.206011	18842.084694	29.999245
429.588095	18877.399155	30.004263
429.923899	18904.229768	30.009280
430.688756	18919.669657	30.014298
430.767561	18952.682228	30.019316
431.634462	18974.421260	30.024333
432.101844	19002.105093	30.029351
432.244859	19016.441010	30.034368
432.984694	19046.477187	30.039386
433.045681	19068.412873	30.044404
433.734179	19087.802918	30.049421
433.910189	19113.563283	30.054439
434.272427	19138.436529	30.059456
434.509890	19158.294989	30.064474
434.932988	19181.852686	30.069492
435.317656	19215.736778	30.074509
435.641906	19240.444189	30.079527
436.123015	19273.148846	30.084544
436.628230	19313.549897	30.089562
436.612848	19336.966272	30.094580
437.159316	19377.510919	30.099597
437.730131	19402.051345	30.104615
438.104982	19453.278555	30.109632
438.898487	19470.836939	30.114650
439.175595	19521.538198	30.119668
439.564145	19544.647209	30.124685
440.091997	19590.079020	30.129703
440.658007	19607.179693	30.134720
441.022107	19646.459165	30.139738
441.114207	19683.907185	30.144756
441.983815	19715.164587	30.149773
442.553712	19737.444165	30.154791
442.672812	19778.206383	30.159808
443.324396	19795.874368	30.164826
443.520270	19840.694022	30.169844
444.365856	19871.522078	30.174861
444.824850	19908.303483	30.179879
444.946240	19929.631509	30.184896
445.562891	19962.166796	30.189914
445.976181	20005.555344	30.194932
446.146745	20027.311917	30.199949
447.076274	20063.648220	30.204967
447.254340	20109.663299	30.209984
447.970005	20128.549102	30.215002
448.381631	20170.786321	30.220020
449.288344	20196.267079	30.225037
449.969150	20212.705591	30.230055
450.094077	20250.794279	30.235072
450.935020	20260.471346	30.240090
450.895449	20283.684316	30.245108
451.537640	20299.679035	30.250125
452.282842	20326.670907	30.255143
452.386070	20348.502836	30.260160
452.992601	20365.714829	30.265178
453.411145	20395.040959	30.270196
453.541780	20422.030118	30.275213
453.890240	20448.212104	30.280231
454.218115	20476.100727	30.285248
454.711890	20500.782341	30.290266
454.990286	20549.589304	30.295284
455.307630	20588.525805	30.300301
455.877500	20608.481199	30.305319
456.159086	20640.175132	30.310336
456.416614	20677.608625	30.315354
456.907382	20710.544707	30.320372
457.180431	20739.207187	30.325389
457.645899	20785.910043	30.330407
458.270130	20813.198442	30.335424
458.955981	20840.495577	30.340442
459.233020	20875.405268	30.345460
459.803671	20910.175331	30.350477
460.644755	20932.021240	30.355495
460.916488	20968.833010	30.360512
461.477580	20995.984132	30.365530
461.707827	21031.771424	30.370548
462.140453	21059.463271	30.375565
462.862345	21083.785404	30.380583
463.124704	21127.435790	30.385600
463.887200	21156.588060	30.390618
463.992798	21172.387242	30.395636
464.270505	21219.817074	30.400653
465.018975	21253.031397	30.405671
465.366636	21284.159726	30.410688
466.014334	21325.093759	30.415706
466.662192	21352.278140	30.420724
466.708735	21374.013426	30.425741
467.547388	21409.442008	30.430759
467.527983	21441.411535	30.435776
468.083368	21479.713412	30.440794
468.764046	21523.531755	30.445812
468.995661	21552.353135	30.450829
469.736390	21577.681076	30.455847
469.942538	21635.264230	30.460864
470.258605	21667.595013	30.465882
470.680296	21703.300963	30.470900
471.430304	21748.987170	30.475917
471.814394	21783.923566	30.480935
472.108999	21824.207550	30.485952
472.729991	21860.200272	30.490970
473.003395	21894.523724	30.495988
473.248249	21948.760291	30.501005
474.029700	21977.546041	30.506023
474.708914	22018.717461	30.511040
474.999031	22057.213432	30.516058
475.870789	22100.315405	30.521076
476.494775	22137.944835	30.526093
477.106966	22160.275478	30.531111
477.443424	22199.829986	30.536128
477.972818	22221.060292	30.541146
478.447685	22257.331589	30.546164
479.055988	22291.710449	30.551181
479.700572	22314.129084	30.556199
479.943388	22360.416882	30.561216
480.698583	22381.127862	30.566234
481.042403	22412.000320	30.571252
481.507850	22451.504195	30.576269
481.939945	22470.277351	30.581287
482.194039	22500.712995	30.586304
482.799045	22524.141611	30.591322
482.974684	22549.347718	30.596340
482.887549	22581.952538	30.601357
483.350691	22606.527758	30.606375
483.996067	22649.897281	30.611392
484.471973	22690.772852	30.616410
484.837302	22728.393709	30.621428
485.618891	22766.912352	30.626445
486.010545	22802.744509	30.631463
486.328521	22843.306971	30.636480
486.914685	22885.484704	30.641498
487.456118	22926.628469	30.646516
487.727169	22970.711429	30.651533
488.159531	23007.545697	30.656551
488.671486	23051.581052	30.661568
489.136944	23100.944233	30.666586
489.654255	23138.099217	30.671604
490.133774	23188.281908	30.676621
490.689896	23208.420021	30.681639
490.925713	23272.721983	30.686656
491.804215	23302.090927	30.691674
492.519166	23333.504652	30.696692
493.111547	23395.800950	30.701709
493.980477	23424.948751	30.706727
493.985512	23464.128396	30.711744
494.682229	23497.381309	30.716762
495.138547	23533.593123	30.721780
495.544483	23566.266341	30.726797
496.207233	23595.697771	30.731815
496.791241	23647.358624	30.736832
496.733918	23679.023665	30.741850
497.886193	23710.242448	30.746868
498.028174	23750.842363	30.751885
498.941643	23783.836872	30.756903
499.368383	23820.646362	30.761920
499.888725	23856.962925	30.766938
500.139599	23884.963195	30.771956
500.567311	23927.680923	30.776973
501.411918	23965.496171	30.781991
501.786472	24001.507840	30.787008
502.060699	24034.685050	30.792026
502.952545	24062.388971	30.797044
503.223972	24113.332389	30.802061
503.947850	24147.295962	30.807079
504.099920	24178.764807	30.812096
504.833092	24214.632399	30.817114
505.435723	24259.032385	30.822132
505.823424	24294.807901	30.827149
506.349258	24327.760539	30.832167
506.650595	24365.351372	30.837184
507.053429	24410.156966	30.842202
507.345807	24442.888677	30.847220
507.650109	24488.280464	30.852237
508.328645	24530.763726	30.857255
508.947967	24552.358570	30.862272
509.430779	24598.899031	30.867290
510.219277	24622.269238	30.872308
510.197359	24682.627563	30.877325
511.177449	24698.391391	30.882343
511.402921	24747.708922	30.887360
511.680419	24771.048114	30.892378
512.589329	24814.789614	30.897396
513.115066	24851.621171	30.902413
513.544268	24889.692272	30.907431
514.049618	24936.524729	30.912448
514.301612	24970.247795	30.917466
515.307469	25008.471506	30.922484
515.626653	25044.867732	30.927501
516.546806	25085.136771	30.932519
516.965420	25123.291252	30.937536
517.220536	25151.064642	30.942554
517.671199	25187.369354	30.947572
517.913671	25240.447813	30.952589
518.314300	25280.048627	30.957607
518.990323	25328.887358	30.962624
519.557328	25357.313280	30.967642
520.155224	25408.999707	30.972660
520.198677	25463.726231	30.977677
521.040857	25498.046444	30.982695
521.360526	25543.563250	30.987712
521.928235	25600.439942	30.992730
522.741149	25638.560414	30.997748
523.044234	25693.232973	31.002765
523.508869	25737.900116	31.007783
524.308626	25776.304237	31.012800
524.872325	25823.297792	31.017818
525.834011	25862.203325	31.022836
526.338449	25906.809458	31.027853
526.920369	25943.418746	31.032871
527.695857	25978.063355	31.037888
527.894915	26019.515455	31.042906
528.778710	26048.634997	31.047924
529.219779	26088.479518	31.052941
529.745256	26120.897101	31.057959
530.441837	26152.202749	31.062976
530.807968	26185.135045	31.067994
531.634426	26222.489842	31.073012
531.339901	26257.061299	31.078029
532.137319	26296.626635	31.083047
532.471877	26336.840872	31.088064
532.990670	26389.240247	31.093082
533.927006	26422.395733	31.098100
533.972172	26465.935102	31.103117
534.620898	26514.469060	31.108135
534.925041	26554.063980	31.113152
535.377699	26598.510917	31.118170
535.765673	26638.935619	31.123188
536.092472	26692.149623	31.128205
536.630211	26735.535631	31.133223
537.516914	26777.554500	31.138240
537.684612	26824.751939	31.143258
538.487498	26869.617301	31.148276
538.827751	26908.605469	31.153293
539.440762	26960.891652	31.158311
539.905692	26997.833957	31.163328
540.378597	27048.509633	31.168346
541.184281	27084.246877	31.173364
541.731697	27140.050613	31.178381
542.304122	27182.551537	31.183399
543.373247	27213.772347	31.188416
543.894264	27257.956547	31.193434
544.688241	27291.795125	31.198452
545.275369	27316.958200	31.203469
545.616771	27354.234553	31.208487
546.040063	27384.226371	31.213504
546.560823	27426.358804	31.218522
547.187465	27466.656972	31.223540
547.469859	27499.914920	31.228557
548.116933	27544.913348	31.233575
549.056636	27580.517693	31.238592
548.996921	27623.159866	31.243610
549.649548	27664.674743	31.248628
550.375241	27707.366144	31.253645
550.756933	27748.778645	31.258663
551.432256	27785.426898	31.263680
552.013575	27839.109160	31.268698
552.450891	27865.098193	31.273716
552.791779	27906.872917	31.278733
553.270848	27948.287752	31.283751
554.244853	27997.136789	31.288768
554.689266	28040.662517	31.293786
555.296942	28070.417463	31.298804
556.000165	28126.303011	31.303821
556.165218	28161.569563	31.308839
556.837787	28212.271462	31.313856
557.362273	28252.516963	31.318874
558.104508	28296.033758	31.323892
558.627775	28349.200672	31.328909
559.378492	28387.253296	31.333927
560.431065	28405.658875	31.338944
560.693710	28467.657167	31.343962
561.463646	28499.969709	31.348980
561.749070	28538.523831	31.353997
562.386119	28570.548834	31.359015
562.785483	28603.686427	31.364032
563.078198	28654.558946	31.369050
564.011640	28682.607009	31.374068
564.647510	28743.484843	31.379085
565.406418	28775.330115	31.384103
565.959956	28802.353189	31.389120
566.230584	28847.358487	31.394138
566.842245	28883.456825	31.399156
567.168062	28921.078863	31.404173
567.388504	28965.893934	31.409191
568.349142	29000.737770	31.414208
568.567268	29049.064316	31.419226
569.366101	29075.785618	31.424244
569.793846	29111.450473	31.429261
570.068962	29155.817711	31.434279
571.291877	29199.072857	31.439296
571.238680	29245.356824	31.444314
571.889664	29264.949341	31.449332
572.634885	29329.894920	31.454349
572.835967	29362.252521	31.459367
573.803466	29403.979370	31.464384
574.070915	29463.665804	31.469402
574.739381	29494.912322	31.474420
574.976577	29541.417196	31.479437
575.551655	29594.891967	31.484455
576.634311	29631.864045	31.489472
577.041540	29682.666396	31.494490
577.656523	29724.880431	31.499508
578.095297	29764.784049	31.504525
579.054865	29803.834213	31.509543
579.568435	29853.386250	31.514560
579.948847	29895.649122	31.519578
581.025576	29937.969818	31.524596
581.395885	29988.169136	31.529613
581.723073	30033.611540	31.534631
582.536239	30064.566632	31.539648
582.844446	30124.017340	31.544666
583.732425	30162.143681	31.549684
584.438946	30207.133751	31.554701
584.737703	30248.937772	31.559719
585.634033	30285.499764	31.564736
585.846735	30339.636705	31.569754
586.426638	30367.433549	31.574772
587.162187	30431.184214	31.579789
587.471992	30473.474016	31.584807
588.473138	30520.963170	31.589824
588.590396	30573.377822	31.594842
589.262590	30623.690188	31.599860
589.935075	30678.486266	31.604877
590.512133	30721.690753	31.609895
591.202507	30771.529466	31.614912
591.709540	30816.307141	31.619930
592.202136	30858.367103	31.624948
593.214251	30913.891564	31.629965
593.803953	30967.477260	31.634983
594.282497	31005.015179	31.640000
594.499268	31055.472332	31.645018
594.672683	31111.359563	31.650036
595.769268	31145.926322	31.655053
596.394809	31217.791942	31.660071
597.078781	31252.783976	31.665088
597.457643	31304.859864	31.670106
597.964314	31368.674285	31.675124
599.083549	31409.553134	31.680141
599.505742	31458.708533	31.685159
600.521259	31480.882379	31.690176
601.029776	31532.080978	31.695194
601.379540	31564.308946	31.700212
602.133869	31596.053315	31.705229
602.467508	31641.648892	31.710247
603.256609	31684.674007	31.715264
603.781019	31737.637476	31.720282
604.003516	31775.758535	31.725300
604.781471	31814.777835	31.730317
604.988476	31875.144661	31.735335
605.932775	31919.193765	31.740352
606.409390	31976.945866	31.745370
606.808441	32023.077410	31.750388
607.571913	32080.377559	31.755405
608.009682	32126.889372	31.760423
608.246244	32183.069657	31.765440
608.850646	32234.174795	31.770458
609.913392	32295.601569	31.775476
610.790080	32347.440720	31.780493
611.224655	32398.809837	31.785511
611.934063	32447.047707	31.790528
612.743014	32489.609970	31.795546
613.259309	32540.172143	31.800564
614.393293	32598.272511	31.805581
614.492190	32645.344127	31.810599
615.255921	32688.793599	31.815616
616.172160	32742.266898	31.820634
616.762038	32784.686711	31.825652
617.526371	32829.706318	31.830669
617.731882	32883.762965	31.835687
618.340073	32920.589535	31.840704
618.987266	32969.669492	31.845722
619.233068	33040.177127	31.850740
619.878845	33082.800015	31.855757
620.630118	33129.185926	31.860775
621.526394	33192.054835	31.865792
621.915736	33243.134312	31.870810
622.608870	33292.751707	31.875828
623.586116	33339.980172	31.880845
624.040344	33393.626893	31.885863
624.487828	33442.732183	31.890880
625.277415	33491.385928	31.895898
625.583434	33550.636613	31.900916
626.203399	33594.284758	31.905933
627.011421	33651.928484	31.910951
627.932294	33691.131245	31.915968
628.718961	33754.084380	31.920986
628.730288	33799.771943	31.926004
630.101039	33852.410404	31.931021
630.471917	33899.522670	31.936039
631.255186	33950.424956	31.941056
631.583143	33989.993972	31.946074
631.959179	34047.752011	31.951092
632.852950	34094.858798	31.956109
633.606813	34148.513845	31.961127
634.211806	34191.533861	31.966144
634.741441	34229.406763	31.971162
635.212037	34278.000133	31.976180
635.812023	34321.238815	31.981197
636.463132	34366.986837	31.986215
636.757639	34426.502581	31.991232
637.660073	34461.767741	31.996250
637.813659	34510.899362	32.001268
638.622991	34566.674971	32.006285
639.125710	34621.982558	32.011303
639.730016	34669.777073	32.016320
640.052273	34727.859738	32.021338
640.833880	34793.677125	32.026356
641.744668	34840.936234	32.031373
642.347443	34902.141737	32.036391
642.621217	34969.719521	32.041408
643.448543	35031.498219	32.046426
644.118545	35097.895775	32.051444
644.555502	35145.841269	32.056461
645.618273	35213.850862	32.061479
646.183682	35276.335842	32.066496
646.844014	35336.493355	32.071514
647.235753	35392.678744	32.076532
648.228613	35457.148817	32.081549
648.812654	35524.643186	32.086567
649.417933	35580.878755	32.091584
650.147327	35638.543490	32.096602
651.046190	35702.745726	32.101620
651.732636	35745.521911	32.106637
652.481253	35799.920908	32.111655
653.366613	35850.155390	32.116672
654.120581	35909.995810	32.121690
654.099450	35970.421777	32.126708
655.253432	36017.249814	32.131725
655.629044	36069.613965	32.136743
655.904763	36135.525102	32.141760
656.980479	36191.452922	32.146778
657.708234	36260.283159	32.151796
658.507139	36312.370991	32.156813
659.397486	36369.881777	32.161831
659.910671	36418.078914	32.166848
660.677686	36469.286317	32.171866
661.024295	36525.016058	32.176884
662.247932	36572.223964	32.181901
662.567938	36615.357119	32.186919
663.007860	36681.061381	32.191936
663.942428	36729.454019	32.196954
664.256897	36790.827452	32.201972
665.100948	36847.175883	32.206989
665.981376	36897.638176	32.212007
666.623911	36973.850569	32.217024
667.593233	37000.388953	32.222042
667.708563	37064.481558	32.227060
668.629623	37106.322076	32.232077
669.010194	37163.544698	32.237095
669.705671	37211.248425	32.242112
670.474218	37261.460035	32.247130
671.149736	37304.962456	32.252148
671.729238	37358.584667	32.257165
672.161472	37403.995925	32.262183
672.610721	37459.315124	32.267200
673.459820	37508.103587	32.272218
673.762157	37576.824092	32.277236
674.815420	37638.704169	32.282253
675.380725	37681.868801	32.287271
675.700980	37748.059823	32.292288
676.588965	37799.493257	32.297306
677.042331	37870.752946	32.302324
678.079936	37929.325639	32.307341
678.328411	37998.450604	32.312359
679.143359	38052.278766	32.317376
680.046099	38119.545225	32.322394
680.346387	38191.396668	32.327412
681.393929	38244.802125	32.332429
681.736374	38300.781228	32.337447
682.174468	38373.057702	32.342464
683.298642	38434.677148	32.347482
684.038589	38516.044696	32.352500
684.567991	38574.290615	32.357517
685.503265	38642.783815	32.362535
685.872042	38717.958190	32.367552
687.037039	38769.467158	32.372570
687.340881	38850.730742	32.377588
688.217993	38902.768438	32.382605
689.270272	38967.559489	32.387623
689.595411	39032.564329	32.392640
690.801837	39096.431005	32.397658
691.599962	39158.644265	32.402676
692.140026	39219.247969	32.407693
692.971882	39275.906069	32.412711
693.566960	39334.396433	32.417728
694.522639	39386.847265	32.422746
695.053905	39447.262396	32.427764
695.907370	39504.441314	32.432781
696.802515	39558.788165	32.437799
697.259392	39611.308078	32.442816
697.520466	39671.259297	32.447834
698.360663	39737.488852	32.452852
698.900757	39789.478871	32.457869
699.562998	39843.488436	32.462887
699.971552	39921.239926	32.467904
700.936190	39972.500638	32.472922
701.509223	40061.991374	32.477940
702.254817	40117.741993	32.482957
703.078764	40181.564864	32.487975
703.764693	40234.184266	32.492992
704.257419	40302.590655	32.498010
705.230623	40371.695061	32.503028
706.138271	40435.511866	32.508045
706.849963	40499.590338	32.513063
707.589607	40560.714234	32.518080
708.147686	40601.518982	32.523098
708.717932	40670.668263	32.528116
709.484686	40721.507021	32.533133
710.248557	40784.105424	32.538151
710.518740	40835.223853	32.543168
710.902125	40895.776486	32.548186
711.747586	40968.943735	32.553204
712.401315	41027.342282	32.558221
713.088096	41092.291110	32.563239
713.696731	41167.323015	32.568256
714.297592	41239.366581	32.573274
715.094699	41308.282053	32.578292
715.876511	41373.295667	32.583309
716.763437	41441.547666	32.588327
717.356495	41508.203514	32.593344
718.326685	41584.498040	32.598362
719.023488	41642.931259	32.603380
719.973397	41716.734804	32.608397
720.691303	41778.908923	32.613415
721.287080	41850.091674	32.618432
722.395195	41907.040998	32.623450
722.695128	41979.605546	32.628468
723.377764	42049.693459	32.633485
724.293791	42110.868944	32.638503
724.949191	42176.687949	32.643520
725.458049	42245.410226	32.648538
726.539081	42324.983281	32.653556
727.274864	42384.753322	32.658573
728.141678	42454.056576	32.663591
728.882069	42516.709221	32.668608
729.662586	42582.588717	32.673626
730.429987	42651.113747	32.678644
730.801033	42725.537391	32.683661
731.786977	42776.894617	32.688679
732.105997	42856.282347	32.693696
732.878818	42917.849399	32.698714
734.031629	42986.030524	32.703732
734.547011	43076.938803	32.708749
735.556330	43124.934076	32.713767
735.891742	43199.201419	32.718784
736.902805	43267.964536	32.723802
738.206969	43330.962528	32.728820
738.642682	43398.556050	32.733837
739.352601	43448.375768	32.738855
740.103453	43523.600365	32.743872
740.827752	43587.350870	32.748890
741.591392	43646.906369	32.753908
742.346524	43715.667859	32.758925
743.111007	43767.804580	32.763943
743.353559	43853.520974	32.768960
744.256973	43913.102454	32.773978
745.157519	43974.577244	32.778996
745.776594	44061.130575	32.784013
746.638437	44114.773277	32.789031
747.251010	44177.944407	32.794048
747.759658	44239.744352	32.799066
748.303849	44304.333719	32.804084
749.132757	44368.502615	32.809101
750.094004	44430.410990	32.814119
750.714260	44512.751988	32.819136
751.472088	44567.664996	32.824154
752.552198	44635.441514	32.829172
752.863827	44699.028382	32.834189
753.619575	44759.576343	32.839207
754.276060	44814.143493	32.844224
755.180516	44882.119288	32.849242
756.029166	44965.703679	32.854260
756.673923	45029.440616	32.859277
757.450282	45093.273557	32.864295
758.070311	45183.406516	32.869312
759.080218	45246.811667	32.874330
759.670333	45317.015912	32.879348
760.317780	45386.558296	32.884365
761.208238	45457.339917	32.889383
761.761695	45530.150313	32.894400
762.495988	45613.437400	32.899418
763.419098	45691.420130	32.904436
764.068476	45771.614091	32.909453
765.090165	45838.177415	32.914471
765.488864	45928.756429	32.919488
766.476789	45996.004007	32.924506
767.283751	46062.826363	32.929524
767.899833	46152.860857	32.934541
768.749223	46228.072031	32.939559
769.318987	46302.091350	32.944576
770.203249	46387.289016	32.949594
770.958646	46467.005531	32.954612
771.884861	46555.159752	32.959629
772.885550	46630.241306	32.964647
773.566672	46701.827943	32.969664
774.294977	46797.993649	32.974682
775.471786	46853.806270	32.979700
775.812306	46937.758640	32.984717
777.104321	47011.167501	32.989735
777.818167	47084.936883	32.994752
778.666261	47157.290700	32.999770
779.599292	47216.733662	33.004788
780.227213	47309.867276	33.009805
781.083743	47365.770377	33.014823
781.849212	47436.488423	33.019840
782.432000	47509.346562	33.024858
783.252651	47576.525887	33.029876
783.690614	47663.138551	33.034893
784.383444	47741.712912	33.039911
785.606439	47813.908794	33.044928
786.056292	47889.910070	33.049946
786.840345	47960.848126	33.054964
787.649874	48043.693081	33.059981
788.670235	48108.873839	33.064999
789.397899	48185.213940	33.070016
789.966563	48254.893848	33.075034
791.172659	48312.132597	33.080052
791.552663	48390.532478	33.085069
792.323350	48448.519351	33.090087
793.072362	48522.109319	33.095104
793.659465	48594.671516	33.100122
794.524101	48664.302772	33.105140
795.036621	48746.412651	33.110157
795.837114	48813.470540	33.115175
796.800031	48898.043119	33.120192
797.346680	48975.264228	33.125210
798.535126	49058.123048	33.130228
799.188234	49140.351211	33.135245
799.769704	49217.798175	33.140263
800.495170	49295.108963	33.145280
801.091456	49375.987301	33.150298
802.173147	49458.047745	33.155316
802.878477	49548.643916	33.160333
804.135437	49641.105952	33.165351
804.879037	49714.386200	33.170368
805.366331	49803.989709	33.175386
806.639923	49883.610806	33.180404
807.441486	49979.962067	33.185421
808.112779	50051.958312	33.190439
809.211971	50129.771773	33.195456
809.781124	50214.870868	33.200474
810.939177	50287.295471	33.205492
811.471749	50372.394831	33.210509
812.516343	50438.119924	33.215527
813.340736	50523.347111	33.220544
814.093245	50609.087889	33.225562
815.343988	50687.737994	33.230580
815.645901	50772.472062	33.235597
816.287880	50838.442592	33.240615
817.318734	50926.280116	33.245632
818.020673	51007.366798	33.250650
818.945131	51085.183851	33.255668
819.718592	51174.960137	33.260685
820.542868	51261.674052	33.265703
821.362076	51340.058064	33.270720
821.992905	51431.593994	33.275738
823.387804	51508.788912	33.280756
823.993861	51592.288733	33.285773
824.766606	51668.415735	33.290791
825.797041	51755.765103	33.295808
826.316772	51830.856939	33.300826
827.047917	51915.824747	33.305844
828.291959	52007.294417	33.310861
829.424773	52073.869888	33.315879
830.409265	52150.801540	33.320896
830.920604	52227.550051	33.325914
831.756987	52283.714880	33.330932
832.732916	52371.186382	33.335949
833.191522	52455.152362	33.340967
834.260682	52514.739760	33.345984
834.936346	52593.896909	33.351002
836.038492	52658.977203	33.356020
836.728835	52730.694017	33.361037
837.511727	52803.892324	33.366055
838.160379	52853.770533	33.371072
838.376892	52934.917953	33.376090
839.493980	53013.138784	33.381108
840.059832	53102.231877	33.386125
840.883087	53170.991017	33.391143
841.776717	53263.744254	33.396160
842.278807	53343.490949	33.401178
843.609915	53425.271128	33.406196
844.194091	53521.133200	33.411213
845.177806	53593.264389	33.416231
846.274644	53686.243102	33.421248
846.266317	53781.531757	33.426266
847.494838	53861.079899	33.431284
848.076870	53956.524849	33.436301
848.714371	54060.353826	33.441319
849.893877	54141.498576	33.446336
850.914713	54249.878866	33.451354
851.671053	54335.106573	33.456372
852.620099	54429.050034	33.461389
853.083942	54519.990671	33.466407
854.345889	54613.080432	33.471424
854.883768	54718.788096	33.476442
856.165457	54812.803697	33.481460
857.128713	54902.524170	33.486477
857.812250	55004.457409	33.491495
859.054947	55092.281554	33.496512
860.397634	55174.048860	33.501530
861.594125	55254.277377	33.506548
862.399721	55345.085683	33.511565
863.190599	55427.390166	33.516583
863.881914	55499.105170	33.521600
864.309139	55580.278237	33.526618
864.990159	55673.765755	33.531636
865.987745	55748.551606	33.536653
866.676345	55853.986195	33.541671
867.371654	55940.632634	33.546688
868.414293	56040.857338	33.551706
869.498555	56124.863847	33.556724
870.282329	56218.003202	33.561741
871.043388	56319.685241	33.566759
871.987806	56398.689963	33.571776
872.673988	56496.748487	33.576794
873.697661	56608.523115	33.581812
874.777346	56689.676182	33.586829
875.674888	56786.749309	33.591847
876.453069	56879.798220	33.596864
877.423316	56967.801024	33.601882
878.117705	57053.474297	33.606900
879.025051	57148.057121	33.611917
879.749318	57239.010888	33.616935
881.098584	57321.014053	33.621952
881.707640	57406.588910	33.626970
882.362259	57495.856682	33.631988
884.053311	57564.810003	33.637005
884.459335	57656.649882	33.642023
885.443435	57712.669105	33.647040
885.903824	57800.419260	33.652058
886.706131	57889.681222	33.657076
887.956128	57967.507597	33.662093
888.547018	58065.251870	33.667111
889.756611	58151.318641	33.672128
890.680840	58235.246636	33.677146
890.925222	58320.564923	33.682164
892.055617	58418.802930	33.687181
892.885848	58502.185159	33.692199
893.614286	58592.494607	33.697216
894.398892	58695.095243	33.702234
895.313709	58792.722359	33.707252
896.183197	58889.391151	33.712269
897.087702	58992.801500	33.717287
898.080723	59076.753938	33.722304
898.965756	59194.280617	33.727322
899.761762	59293.839321	33.732340
901.048137	59383.321915	33.737357
901.768583	59489.517336	33.742375
902.898598	59587.253305	33.747392
903.487698	59695.223026	33.752410
904.561096	59786.919910	33.757428
905.753168	59893.614037	33.762445
906.274699	59994.258895	33.767463
907.281194	60094.280918	33.772480
908.342351	60189.167391	33.777498
909.126068	60300.045898	33.782516
910.133452	60384.579744	33.787533
911.123745	60491.322036	33.792551
911.841610	60592.276710	33.797568
912.995562	60685.944847	33.802586
913.834739	60799.144455	33.807604
914.797643	60885.787296	33.812621
915.292274	61002.595012	33.817639
916.394382	61084.859419	33.822656
917.688897	61191.866728	33.827674
918.562716	61300.716081	33.832692
919.540039	61385.912835	33.837709
920.542805	61492.371530	33.842727
921.737067	61578.725009	33.847744
922.405359	61683.990808	33.852762
923.280846	61783.584882	33.857780
924.407093	61876.856070	33.862797
925.195484	61973.417982	33.867815
926.065999	62054.681508	33.872832
927.174313	62162.216570	33.877850
927.814522	62263.224178	33.882868
929.209884	62360.654563	33.887885
930.200493	62451.746168	33.892903
931.160876	62530.076633	33.897920
931.917541	62606.339994	33.902938
932.571548	62685.247187	33.907956
933.477620	62774.373941	33.912973
934.353628	62854.187507	33.917991
935.154512	62949.186214	33.923008
935.823041	63042.494966	33.928026
936.475533	63140.379157	33.933044
937.801353	63232.343258	33.938061
938.335871	63333.266048	33.943079
939.540818	63425.891355	33.948096
940.267477	63540.300070	33.953114
941.385303	63633.622347	33.958132
942.160950	63731.783679	33.963149
942.975183	63852.265524	33.968167
944.239509	63941.934457	33.973184
945.165634	64042.741869	33.978202
945.695084	64151.397213	33.983220
946.966725	64258.390847	33.988237
947.818737	64370.397218	33.993255
948.603558	64475.688449	33.998272
949.816090	64587.809265	34.003290
950.942166	64687.265082	34.008308
951.983086	64793.663681	34.013325
953.050852	64902.566092	34.018343
953.630070	65003.086409	34.023360
954.978263	65113.852877	34.028378
955.534924	65219.582442	34.033396
956.471098	65320.098160	34.038413
957.503124	65424.628933	34.043431
958.529997	65538.831355	34.048448
959.669735	65657.794814	34.053466
960.434949	65763.314186	34.058484
961.433800	65873.145814	34.063501
962.616730	65988.377772	34.068519
963.255010	66086.440444	34.073536
964.887122	66197.035370	34.078554
965.676558	66301.675856	34.083572
966.718533	66401.738262	34.088589
967.777920	66519.835536	34.093607
968.733470	66623.210127	34.098624
969.576064	66729.988994	34.103642
970.474218	66831.538838	34.108660
972.077463	66928.043641	34.113677
972.615876	67035.646406	34.118695
973.698767	67140.415319	34.123712
974.611075	67245.853105	34.128730
975.691436	67346.463887	34.133748
976.318937	67443.698205	34.138765
977.621340	67556.997054	34.143783
978.417703	67654.973080	34.148800
979.053877	67765.609153	34.153818
980.205396	67876.890326	34.158836
981.053727	67977.569741	34.163853
981.718480	68086.251115	34.168871
982.938956	68185.608974	34.173888
983.864856	68276.113277	34.178906
984.989653	68398.962183	34.183924
986.076880	68484.994457	34.188941
986.996581	68588.628492	34.193959
988.000631	68686.601963	34.198976
989.073060	68781.526398	34.203994
989.536185	68891.678405	34.209012
990.806737	68989.920558	34.214029
991.758470	69107.993922	34.219047
992.472338	69203.419688	34.224064
993.438127	69304.535842	34.229082
994.411235	69431.584985	34.234100
995.428540	69534.861067	34.239117
996.492860	69629.835155	34.244135
997.624349	69743.341388	34.249152
999.015933	69851.411576	34.254170
999.637360	69965.442491	34.259188
1000.690842	70077.509996	34.264205
1001.831174	70185.697821	34.269223
1002.426362	70296.942367	34.274240
1003.630508	70413.340828	34.279258
1004.477547	70524.868812	34.284276
1005.682343	70645.248843	34.289293
1006.359607	70757.399048	34.294311
1007.794322	70862.580636	34.299328
1008.959552	70982.501497	34.304346
1009.739634	71103.615309	34.309364
1011.005749	71198.413272	34.314381
1012.013335	71323.415811	34.319399
1012.885177	71436.322390	34.324416
1014.440633	71542.530918	34.329434
1015.458348	71657.165713	34.334452
1016.300641	71761.207977	34.339469
1017.396664	71876.292826	34.344487
1018.723683	71998.007508	34.349504
1019.657195	72097.140273	34.354522
1020.299688	72213.973628	34.359540
1021.620705	72310.897538	34.364557
1022.431175	72414.480739	34.369575
1023.404294	72541.259349	34.374592
1024.541651	72650.579595	34.379610
1025.526069	72772.606296	34.384628
1026.604104	72866.330119	34.389645
1027.648311	72990.345351	34.394663
1028.269932	73097.532241	34.399680
1029.765879	73210.286478	34.404698
1030.414014	73327.915349	34.409716
1031.540496	73430.366746	34.414733
1032.632530	73552.324250	34.419751
1033.328577	73673.896853	34.424768
1034.695809	73783.079346	34.429786
1035.461776	73908.566337	34.434804
1036.339067	74029.524609	34.439821
1037.399229	74142.454563	34.444839
1038.205995	74247.494978	34.449856
1039.335926	74346.683558	34.454874
1040.094596	74464.143569	34.459892
1041.574108	74582.892465	34.464909
1042.797860	74693.012733	34.469927
1043.533160	74813.827720	34.474944
1044.724934	74911.953947	34.479962
1045.409955	75021.340211	34.484980
1046.676763	75135.399344	34.489997
1047.658168	75248.076336	34.495015
1048.940666	75361.849888	34.500032
1049.740724	75482.728116	34.505050
1050.891680	75604.530780	34.510068
1051.536962	75713.086634	34.515085
1052.995253	75838.279674	34.520103
1053.727746	75969.617901	34.525120
1054.601615	76082.392512	34.530138
1055.759680	76207.073151	34.535156
1056.801827	76335.217276	34.540173
1057.894417	76456.686791	34.545191
1058.720964	76573.320437	34.550208
1060.065709	76707.751276	34.555226
1060.919572	76839.183290	34.560244
1062.416631	76968.763211	34.565261
1063.916046	77081.222693	34.570279
1064.773414	77207.385658	34.575296
1065.888332	77330.316798	34.580314
1067.063951	77461.278220	34.585332
1068.034788	77584.669908	34.590349
1069.182145	77699.849612	34.595367
1070.244260	77825.693121	34.600384
1071.499628	77942.051542	34.605402
1072.488800	78067.345645	34.610420
1073.377178	78199.703741	34.615437
1074.800535	78319.589636	34.620455
1075.738466	78431.210493	34.625472
1076.616573	78563.736917	34.630490
1078.094515	78688.009018	34.635508
1078.946800	78805.985012	34.640525
1080.324372	78932.379305	34.645543
1080.950370	79065.467371	34.650560
1082.370242	79172.249871	34.655578
1083.093350	79300.811075	34.660596
1083.832918	79442.094099	34.665613
1085.239919	79562.874793	34.670631
1086.278007	79697.563775	34.675648
1087.479319	79822.619982	34.680666
1088.812550	79938.566530	34.685684
1089.801413	80062.697216	34.690701
1090.813140	80190.472210	34.695719
1091.747438	80329.397922	34.700736
1093.097408	80454.623956	34.705754
1094.010416	80581.386745	34.710772
1095.229316	80712.014434	34.715789
1096.324825	80814.779944	34.720807
1097.185641	80946.578595	34.725824
1098.499441	81065.581394	34.730842
1099.183741	81185.803869	34.735860
1100.469657	81301.405298	34.740877
1101.640390	81412.505936	34.745895
1102.427766	81535.248900	34.750912
1103.612508	81654.787646	34.755930
1104.505467	81776.244639	34.760948
1105.324806	81905.533729	34.765965
1106.866174	82031.788238	34.770983
1107.419758	82167.392180	34.776000
1108.979832	82299.303141	34.781018
1109.853839	82423.605331	34.786036
1111.067965	82563.563550	34.791053
1112.175935	82690.270289	34.796071
1113.047194	82828.034283	34.801088
1114.605875	82954.139910	34.806106
1115.734663	83091.339971	34.811124
1116.598850	83233.684781	34.816141
1117.989544	83363.081690	34.821159
1119.112411	83493.249024	34.826176
1120.143994	83626.516825	34.831194
1121.308989	83767.597272	34.836212
1122.123154	83896.880546	34.841229
1123.774238	84038.764276	34.846247
1124.721345	84182.765058	34.851264
1126.300442	84309.039976	34.856282
1127.796169	84436.308862	34.861300
1128.771077	84554.911306	34.866317
1130.463127	84670.675440	34.871335
1131.563724	84797.712206	34.876352
1132.549122	84925.166369	34.881370
1133.518795	85048.052683	34.886388
1134.701799	85173.162905	34.891405
1135.828005	85301.595895	34.896423
1136.817646	85429.469711	34.901440
1138.166506	85552.203810	34.906458
1139.237952	85678.434893	34.911476
1140.071118	85819.879010	34.916493
1141.515723	85940.874047	34.921511
1142.603990	86078.719639	34.926528
1143.597923	86202.645722	34.931546
1144.471612	86327.204964	34.936564
1145.645787	86475.737672	34.941581
1146.745757	86606.408379	34.946599
1147.470095	86755.956693	34.951616
1148.963682	86885.630718	34.956634
1150.114985	87020.095909	34.961652
1151.315137	87178.145526	34.966669
1152.405275	87312.059529	34.971687
1153.501961	87444.095356	34.976704
1154.587955	87588.640958	34.981722
1155.819766	87718.557691	34.986740
1156.892208	87858.345880	34.991757
1158.285149	87992.456267	34.996775
1159.229567	88128.605383	35.001792
1160.073819	88255.943845	35.006810
1161.765209	88377.071534	35.011828
1162.542813	88510.916258	35.016845
1163.738338	88638.492002	35.021863
1164.911044	88779.041700	35.026880
1166.112245	88908.553143	35.031898
1167.280596	89037.823967	35.036916
1168.249618	89167.690069	35.041933
1169.715914	89303.276695	35.046951
1170.636678	89438.343849	35.051968
1171.749987	89580.659885	35.056986
1173.186558	89703.283696	35.062004
1174.045342	89855.703194	35.067021
1175.059535	89989.487832	35.072039
1176.429225	90140.613898	35.077056
1177.517137	90285.664216	35.082074
1178.539393	90428.898300	35.087092
1179.684538	90576.218101	35.092109
1180.881606	90712.836585	35.097127
1181.951649	90861.548912	35.102144
1183.346644	91007.813713	35.107162
1184.529721	91161.980534	35.112180
1186.026307	91303.867446	35.117197
1187.038745	91455.913225	35.122215
1188.313765	91595.003967	35.127232
1189.557320	91733.600970	35.132250
1190.647526	91881.539130	35.137268
1191.914230	92028.963236	35.142285
1193.258151	92172.473825	35.147303
1194.116181	92322.557943	35.152320
1195.687311	92470.923240	35.157338
1197.210435	92624.711074	35.162356
1198.053549	92774.579283	35.167373
1199.656408	92917.579208	35.172391
1201.061873	93064.975545	35.177408
1202.024306	93205.865503	35.182426
1203.306679	93348.887562	35.187444
1204.369483	93489.725420	35.192461
1205.765634	93622.895944	35.197479
1206.881247	93794.352709	35.202496
1208.195157	93915.621801	35.207514
1209.479135	94053.841145	35.212532
1210.578460	94217.283595	35.217549
1211.643277	94366.292415	35.222567
1212.792851	94523.454579	35.227584
1214.002384	94654.668535	35.232602
1215.451988	94807.123300	35.237620
1216.408113	94960.840410	35.242637
1217.739140	95095.263555	35.247655
1218.947814	95251.953382	35.252672
1219.892800	95417.649390	35.257690
1221.666575	95552.397065	35.262708
1222.616137	95698.833337	35.267725
1223.735561	95844.370630	35.272743
1225.226344	95979.722524	35.277760
1226.144227	96113.641850	35.282778
1227.714632	96236.546426	35.287796
1228.801056	96386.425570	35.292813
1229.707736	96525.618456	35.297831
1230.814945	96670.606377	35.302848
1231.871572	96800.168232	35.307866
1233.213341	96934.025043	35.312884
1234.134362	97084.295703	35.317901
1235.399202	97235.866451	35.322919
1236.729966	97391.400462	35.327936
1237.937468	97546.455383	35.332954
1239.278560	97684.529894	35.337972
1240.259677	97843.943562	35.342989
1241.190432	98009.218064	35.348007
1242.349657	98169.504016	35.353024
1243.457190	98341.376377	35.358042
1244.907971	98492.590672	35.363060
1246.211065	98667.344504	35.368077
1247.493518	98828.273443	35.373095
1248.841996	98981.898632	35.378112
1249.976755	99156.499509	35.383130
1251.531237	99309.562725	35.388148
1252.519257	99475.363855	35.393165
1254.158627	99635.843163	35.398183
1255.604394	99803.503511	35.403200
1256.493541	99976.998241	35.408218
1258.334724	100126.630216	35.413236
1259.329401	100292.942338	35.418253
1260.539015	100450.711879	35.423271
1261.810367	100619.424534	35.428288
1263.246544	100786.922755	35.433306
1264.678942	100934.828130	35.438324
1265.727792	101111.868107	35.443341
1266.787057	101273.760767	35.448359
1268.236191	101436.554299	35.453376
1269.545493	101612.803773	35.458394
1271.075960	101767.399351	35.463412
1271.986870	101939.013528	35.468429
1273.153647	102100.065997	35.473447
1274.730719	102276.233647	35.478464
1276.090810	102441.788128	35.483482
1277.705018	102600.077457	35.488500
1278.853628	102775.140097	35.493517
1280.096658	102922.151781	35.498535
1281.674208	103081.658764	35.503552
1282.732115	103253.866698	35.508570
1284.331800	103407.709177	35.513588
1285.683916	103568.204465	35.518605
1286.557676	103729.510917	35.523623
1288.157923	103883.198235	35.528640
1289.538462	104053.247271	35.533658
1290.618761	104206.475171	35.538676
1291.715144	104364.409475	35.543693
1292.766414	104518.371728	35.548711
1294.222647	104674.599309	35.553728
1295.426640	104830.918648	35.558746
1296.850196	104969.308328	35.563764
1297.704656	105118.559731	35.568781
1298.835086	105280.038488	35.573799
1300.518041	105426.761756	35.578816
1301.651844	105582.552995	35.583834
1303.247540	105734.164780	35.588852
1304.730457	105892.819892	35.593869
1306.073686	106042.398092	35.598887
1307.376989	106188.180214	35.603904
1308.194477	106366.359791	35.608922
1309.528421	106528.827234	35.613940
1310.993424	106678.877367	35.618957
1311.937917	106842.142961	35.623975
1312.946535	107007.823335	35.628992
1314.029522	107175.859949	35.634010
1315.530222	107354.773665	35.639028
1316.837661	107530.934789	35.644045
1318.315854	107709.373742	35.649063
1319.803036	107888.445477	35.654080
1320.820386	108073.776558	35.659098
1322.068852	108241.047508	35.664116
1323.671973	108417.073183	35.669133
1324.501797	108600.862206	35.674151
1326.138396	108782.492745	35.679168
1327.684219	108961.303630	35.684186
1328.833208	109154.476519	35.689204
1330.219140	109346.144902	35.694221
1331.551676	109512.360627	35.699239
1333.216375	109684.961600	35.704256
1334.160104	109875.020848	35.709274
1335.640469	110062.249312	35.714292
1337.192985	110238.530442	35.719309
1338.400085	110426.064643	35.724327
1339.958382	110610.341705	35.729344
1341.011423	110800.011003	35.734362
1342.480497	110976.025883	35.739380
1343.771957	111164.482789	35.744397
1345.091760	111348.986877	35.749415
1346.603509	111525.986359	35.754432
1347.871274	111726.908370	35.759450
1349.118190	111913.669041	35.764468
1350.845722	112097.835417	35.769485
1351.926697	112284.922781	35.774503
1353.690423	112467.509996	35.779520
1354.983696	112655.883067	35.784538
1356.176564	112838.044686	35.789556
1357.487269	113032.216239	35.794573
1358.642750	113211.056867	35.799591
1360.670736	113391.178078	35.804608
1361.718929	113576.729479	35.809626
1362.730817	113769.669230	35.814644
1364.358227	113954.884496	35.819661
1365.665520	114137.043764	35.824679
1367.625797	114299.912834	35.829696
1368.520609	114479.152161	35.834714
1369.911339	114636.422793	35.839732
1371.550371	114804.796838	35.844749
1372.714252	114967.410663	35.849767
1374.341820	115130.939430	35.854784
1375.519191	115307.803731	35.859802
1376.747351	115472.696005	35.864820
1378.362984	115643.871266	35.869837
1379.680985	115818.703594	35.874855
1380.668091	115991.272606	35.879872
1381.908634	116172.134063	35.884890
1383.294563	116343.103660	35.889908
1384.784522	116519.825465	35.894925
1385.845007	116709.361256	35.899943
1387.303022	116891.218912	35.904960
1388.816985	117081.147574	35.909978
1390.017347	117275.375756	35.914996
1391.385709	117461.968509	35.920013
1392.967956	117651.852581	35.925031
1394.462793	117847.975702	35.930048
1395.696948	118039.975677	35.935066
1397.038334	118232.270290	35.940084
1398.655604	118418.710159	35.945101
1399.676848	118623.962228	35.950119
1401.220074	118821.775630	35.955136
1402.512994	119022.004708	35.960154
1403.934324	119225.102196	35.965172
1405.117604	119413.891329	35.970189
1406.516411	119625.790367	35.975207
1407.850828	119835.022992	35.980224
1409.178656	120048.690695	35.985242
1410.809193	120249.939377	35.990260
1412.660833	120446.696738	35.995277
1413.908179	120658.615610	36.000295
1415.468563	120854.852456	36.005312
1417.021993	121067.846792	36.010330
1418.469748	121278.212791	36.015348
1420.161290	121472.014520	36.020365
1421.358673	121675.584654	36.025383
1423.059489	121870.869620	36.030400
1424.233575	122076.979511	36.035418
1426.160661	122274.245221	36.040436
1427.499096	122467.211198	36.045453
1428.739784	122683.269944	36.050471
1430.330186	122876.414177	36.055488
1432.041487	123072.719598	36.060506
1433.189418	123269.698611	36.065524
1434.732996	123463.931128	36.070541
1435.922339	123673.103417	36.075559
1437.410478	123861.635473	36.080576
1439.070615	124065.669762	36.085594
1440.365336	124273.094806	36.090612
1442.352562	124450.203099	36.095629
1443.497231	124655.375084	36.100647
1445.047587	124832.732660	36.105664
1446.307320	125007.224364	36.110682
1447.465502	125183.316627	36.115700
1449.105211	125360.942156	36.120717
1450.762515	125537.324749	36.125735
1451.939821	125717.318742	36.130752
1453.345146	125907.195677	36.135770
1454.620102	126090.330634	36.140788
1456.196951	126271.721506	36.145805
1456.919034	126472.908447	36.150823
1458.505541	126666.333988	36.155840
1459.949592	126858.947517	36.160858
1461.263801	127069.393095	36.165876
1462.711661	127267.430466	36.170893
1464.118471	127480.638640	36.175911
1465.680328	127667.602191	36.180928
1466.428421	127894.485116	36.185946
1468.341447	128106.655000	36.190964
1470.059702	128307.494500	36.195981
1471.400583	128528.473978	36.200999
1472.970982	128734.837948	36.206016
1474.377954	128946.131968	36.211034
1475.775121	129179.737775	36.216052
1477.339237	129390.136123	36.221069
1478.710859	129616.680800	36.226087
1480.076062	129825.112461	36.231104
1481.552080	130052.049499	36.236122
1483.203553	130278.200392	36.241140
1484.889598	130494.732044	36.246157
1486.357136	130724.703749	36.251175
1487.882486	130942.037209	36.256192
1489.456412	131170.019319	36.261210
1490.962595	131388.588193	36.266228
1492.559082	131612.794912	36.271245
1493.775290	131836.050295	36.276263
1495.527199	132042.815386	36.281280
1497.146002	132266.745045	36.286298
1498.294822	132496.807253	36.291316
1500.245900	132711.552825	36.296333
1501.549498	132950.538976	36.301351
1503.236767	133168.712785	36.306368
1504.753654	133383.101656	36.311386
1506.449243	133611.033482	36.316404
1507.894813	133829.491497	36.321421
1509.503680	134055.730175	36.326439
1511.043964	134274.429954	36.331456
1512.609232	134487.514384	36.336474
1514.290489	134713.797447	36.341492
1515.955349	134929.036015	36.346509
1517.596412	135143.823826	36.351527
1518.963802	135354.589354	36.356544
1520.773763	135566.249105	36.361562
1522.107069	135783.498071	36.366580
1524.132766	135997.889011	36.371597
1525.519385	136204.412829	36.376615
1527.196054	136397.663112	36.381632
1528.288147	136580.338187	36.386650
1529.473651	136777.597183	36.391668
1531.407634	136971.317260	36.396685
1532.616259	137162.708225	36.401703
1533.889050	137370.259463	36.406720
1535.385540	137559.161631	36.411738
1536.689350	137778.609734	36.416756
1538.132603	137976.368090	36.421773
1539.702452	138189.871820	36.426791
1541.327921	138394.713120	36.431808
1542.544440	138611.469444	36.436826
1543.657140	138849.875695	36.441844
1545.488375	139050.316862	36.446861
1546.801026	139283.803246	36.451879
1548.132124	139502.993710	36.456896
1549.934660	139734.631630	36.461914
1551.214430	139971.550299	36.466932
1553.014315	140203.559801	36.471949
1554.424131	140440.512222	36.476967
1555.823132	140670.954205	36.481984
1557.651298	140906.690590	36.487002
1559.207820	141155.652328	36.492020
1560.959851	141384.142687	36.497037
1562.725709	141620.224073	36.502055
1563.884800	141859.280630	36.507072
1566.118960	142069.943726	36.512090
1567.830378	142316.748560	36.517108
1569.498088	142548.024019	36.522125
1570.906573	142774.906485	36.527143
1572.885215	142996.782483	36.532160
1574.432972	143235.788125	36.537178
1575.975603	143465.239967	36.542196
1577.423195	143698.054687	36.547213
1579.123061	143937.827462	36.552231
1580.412533	144171.076472	36.557248
1582.421393	144405.657894	36.562266
1584.063528	144643.772270	36.567284
1585.557312	144872.443852	36.572301
1586.970923	145104.868999	36.577319
1588.560176	145347.598233	36.582336
1590.155372	145576.398323	36.587354
1591.641246	145823.989639	36.592372
1593.145753	146055.773686	36.597389
1594.701421	146294.358087	36.602407
1595.777198	146531.854378	36.607424
1597.937593	146776.468721	36.612442
1599.147950	147026.407619	36.617460
1600.595252	147261.961712	36.622477
1602.239893	147517.742502	36.627495
1603.815636	147776.920833	36.632512
1606.333409	148004.020233	36.637530
1607.500359	148270.898624	36.642548
1609.235986	148514.795292	36.647565
1611.095124	148745.148366	36.652583
1612.518896	148974.431362	36.657600
1614.198616	149187.854834	36.662618
1615.882645	149411.521882	36.667636
1617.628268	149613.186348	36.672653
1618.960185	149837.951799	36.677671
1620.534454	150061.894347	36.682688
1622.302269	150283.348348	36.687706
1623.795961	150521.581329	36.692724
1625.398238	150729.842349	36.697741
1627.038283	150967.079209	36.702759
1628.365744	151197.521611	36.707776
1629.963499	151427.605774	36.712794
1631.351927	151659.956076	36.717812
1633.195113	151895.785571	36.722829
1634.693571	152154.288795	36.727847
1635.839536	152387.697002	36.732864
1637.798134	152621.117253	36.737882
1639.432706	152884.891344	36.742900
1640.941647	153130.735126	36.747917
1642.949526	153383.854916	36.752935
1644.427053	153632.103615	36.757952
1646.250029	153881.503762	36.762970
1647.881673	154132.533673	36.767988
1649.397540	154373.631083	36.773005
1651.385710	154614.667899	36.778023
1652.778470	154888.588619	36.783040
1654.886036	155123.663735	36.788058
1656.067537	155378.565500	36.793076
1657.875142	155645.947496	36.798093
1659.983910	155897.320572	36.803111
1661.309627	156151.444511	36.808128
1662.881396	156415.383220	36.813146
1664.526913	156664.350383	36.818164
1666.376783	156920.603072	36.823181
1668.209695	157185.850322	36.828199
1669.651147	157448.321514	36.833216
1671.336046	157701.639172	36.838234
1673.107918	157978.250799	36.843252
1674.645402	158237.327196	36.848269
1676.657436	158498.663335	36.853287
1678.120067	158753.393489	36.858304
1679.863133	159021.712433	36.863322
1681.707738	159283.207883	36.868340
1683.548167	159533.090519	36.873357
1685.332827	159792.468969	36.878375
1686.892551	160061.509793	36.883392
1688.611663	160316.083827	36.888410
1690.935188	160570.994874	36.893428
1692.054635	160821.876186	36.898445
1694.162439	161066.325146	36.903463
1695.718531	161329.885296	36.908480
1697.340908	161580.501902	36.913498
1698.870209	161845.021233	36.918516
1700.733693	162090.771516	36.923533
1702.440122	162338.818444	36.928551
1703.782501	162589.537335	36.933568
1705.532393	162821.424214	36.938586
1707.065722	163066.979995	36.943604
1708.503809	163299.934026	36.948621
1710.877347	163550.369050	36.953639
1712.010326	163793.456943	36.958656
1713.626718	164036.736027	36.963674
1715.501924	164281.827258	36.968692
1717.150572	164529.657466	36.973709
1718.633157	164779.747844	36.978727
1720.076710	165043.099408	36.983744
1722.025481	165294.755328	36.988762
1723.799855	165551.995706	36.993780
1725.407290	165820.260405	36.998797
1727.415967	166079.306269	37.003815
1728.728963	166343.968844	37.008832
1730.289935	166605.803649	37.013850
1732.200824	166872.302881	37.018868
1733.805906	167146.170833	37.023885
1735.713842	167404.201902	37.028903
1737.355126	167694.645292	37.033920
1739.387585	167967.601597	37.038938
1741.022992	168236.006079	37.043956
1743.161935	168504.700345	37.048973
1744.843209	168761.394186	37.053991
1746.757154	169039.133491	37.059008
1748.309975	169322.373607	37.064026
1750.111365	169590.786690	37.069044
1751.883131	169861.311940	37.074061
1754.039105	170130.560403	37.079079
1755.555955	170416.947349	37.084096
1757.418490	170685.967238	37.089114
1759.366780	170954.797802	37.094132
1760.989662	171233.296859	37.099149
1763.030531	171503.435732	37.104167
1764.952714	171768.521398	37.109184
1766.279285	172033.754175	37.114202
1768.312881	172315.671420	37.119220
1769.804425	172597.245463	37.124237
1771.477560	172865.612793	37.129255
1773.230382	173159.745750	37.134272
1775.181642	173434.402734	37.139290
1777.296989	173704.405384	37.144308
1778.751620	173988.088285	37.149325
1780.747993	174260.942473	37.154343
1782.719091	174540.487903	37.159360
1783.928238	174818.849619	37.164378
1786.031359	175090.855246	37.169396
1788.121474	175386.968113	37.174413
1789.727126	175644.391473	37.179431
1791.419511	175924.371332	37.184448
1793.473193	176212.516435	37.189466
1795.285871	176476.673957	37.194484
1796.844345	176763.518762	37.199501
1798.940039	177030.984140	37.204519
1800.667396	177285.493323	37.209536
1802.388608	177538.178178	37.214554
1803.938725	177801.206043	37.219572
1805.739352	178051.585131	37.224589
1807.535545	178306.863564	37.229607
1809.446776	178579.087757	37.234624
1811.263310	178826.601728	37.239642
1813.110019	179081.826133	37.244660
1814.533104	179353.777621	37.249677
1816.469535	179615.930919	37.254695
1818.532342	179884.701266	37.259712
1820.225227	180155.866534	37.264730
1821.942418	180432.459931	37.269748
1823.353005	180712.960827	37.274765
1825.816723	180973.617793	37.279783
1827.279570	181255.103587	37.284800
1829.085235	181530.675022	37.289818
1831.001666	181806.725464	37.294836
1832.768363	182097.341890	37.299853
1834.429503	182367.866407	37.304871
1836.285711	182654.577113	37.309888
1837.916245	182942.987691	37.314906
1839.831681	183235.047248	37.319924
1841.367388	183525.011999	37.324941
1843.650447	183808.465018	37.329959
1845.328254	184102.407886	37.334976
1847.315476	184397.661275	37.339994
1849.544152	184682.955696	37.345012
1851.332878	184982.228741	37.350029
1852.716699	185270.922062	37.355047
1855.110199	185557.528237	37.360064
1857.158905	185857.996688	37.365082
1859.102858	186142.102059	37.370100
1860.698987	186443.382212	37.375117
1862.974760	186722.286713	37.380135
1864.859192	187012.256751	37.385152
1866.410343	187314.729914	37.390170
1868.755929	187607.891719	37.395188
1870.568164	187895.594677	37.400205
1872.155406	188189.464277	37.405223
1874.179653	188495.144033	37.410240
1876.240911	188772.749889	37.415258
1878.087580	189058.766834	37.420276
1880.395043	189348.544777	37.425293
1882.762133	189626.310194	37.430311
1884.444693	189903.970170	37.435328
1886.408929	190186.599722	37.440346
1888.709942	190454.710516	37.445364
1890.396590	190736.245269	37.450381
1892.351301	191012.954820	37.455399
1894.006865	191289.485021	37.460416
1896.254700	191576.887513	37.465434
1898.127380	191835.771796	37.470452
1899.496754	192136.654979	37.475469
1901.533395	192389.475386	37.480487
1903.274985	192659.489362	37.485504
1904.689560	192919.936966	37.490522
1906.930037	193174.683498	37.495540
1908.345332	193436.593201	37.500557
1909.872984	193696.658931	37.505575
1912.054055	193968.869377	37.510592
1913.529635	194245.774857	37.515610
1915.600570	194516.584356	37.520628
1917.259763	194797.436161	37.525645
1919.331000	195086.524407	37.530663
1921.051297	195376.152293	37.535680
1922.691329	195659.436047	37.540698
1925.006258	195942.309669	37.545716
1926.714928	196243.468467	37.550733
1928.304380	196540.129646	37.555751
1930.573832	196833.042024	37.560768
1932.137025	197130.421530	37.565786
1934.525362	197439.056624	37.570804
1936.337546	197741.426205	37.575821
1938.561079	198035.164980	37.580839
1940.885503	198338.916343	37.585856
1942.420626	198641.132026	37.590874
1944.419948	198936.688374	37.595892
1946.364689	199244.147961	37.600909
1948.558614	199545.743867	37.605927
1950.424008	199850.477946	37.610944
1952.314316	200164.120134	37.615962
1954.385680	200463.887524	37.620980
1956.051553	200772.123642	37.625997
1958.047007	201081.350036	37.631015
1960.174435	201389.554494	37.636032
1961.794909	201731.896828	37.641050
1964.097996	202018.320914	37.646068
1966.270332	202345.043008	37.651085
1967.993564	202656.136623	37.656103
1970.480585	202971.731179	37.661120
1971.926033	203294.182283	37.666138
1974.167809	203596.719600	37.671156
1976.096439	203923.743487	37.676173
1978.128720	204237.360953	37.681191
1980.322238	204551.030728	37.686208
1982.183247	204878.718230	37.691226
1984.237664	205189.417835	37.696244
1986.432821	205508.855637	37.701261
1988.183875	205824.874812	37.706279
1990.206682	206150.055827	37.711296
1992.219946	206464.259686	37.716314
1994.332699	206785.063157	37.721332
1996.298671	207104.507985	37.726349
1998.577294	207417.189588	37.731367
2000.858630	207737.019394	37.736384
2002.054402	208055.994912	37.741402
2004.531296	208360.030404	37.746420
2006.479693	208681.492210	37.751437
2008.563812	208983.892083	37.756455
2010.688875	209278.403497	37.761472
2012.675496	209577.546531	37.766490
2014.498994	209849.067382	37.771508
2016.737185	210146.434066	37.776525
2018.677840	210427.079252	37.781543
2020.736933	210712.378706	37.786560
2022.378442	211004.258335	37.791578
2024.364323	211302.952787	37.796596
2026.001591	211603.824081	37.801613
2028.195478	211901.485436	37.806631
2030.115636	212202.276597	37.811648
2031.792928	212522.227056	37.816666
2034.165058	212829.208308	37.821684
2035.922036	213136.720273	37.826701
2038.131963	213455.752944	37.831719
2039.991790	213771.706889	37.836736
2041.954260	214106.321533	37.841754
2043.858886	214407.976006	37.846772
2046.391583	214740.713284	37.851789
2048.236707	215061.106596	37.856807
2050.749779	215396.351361	37.861824
2052.311404	215714.748718	37.866842
2054.497380	216045.033659	37.871860
2056.312506	216375.620271	37.876877
2058.583555	216713.334921	37.881895
2060.917257	217030.206643	37.886912
2062.675014	217382.555979	37.891930
2064.703841	217708.023830	37.896948
2067.120806	218040.744796	37.901965
2068.918233	218380.409070	37.906983
2071.190164	218710.934312	37.912000
2073.320191	219062.445812	37.917018
2075.395840	219390.034318	37.922036
2077.414413	219727.016298	37.927053
2079.558345	220074.429468	37.932071
2082.121304	220399.164618	37.937088
2083.984792	220746.714353	37.942106
2086.255655	221081.161250	37.947124
2088.426059	221431.014458	37.952141
2090.366473	221761.707709	37.957159
2092.544804	222103.398538	37.962176
2094.681997	222455.217151	37.967194
2097.025944	222786.879346	37.972212
2098.892691	223126.744996	37.977229
2101.029184	223476.689200	37.982247
2103.610789	223806.223005	37.987264
2105.292124	224154.020400	37.992282
2107.413048	224484.176131	37.997300
2109.643695	224810.544635	38.002317
2111.669453	225216.561556	38.007335
2114.157534	225545.647626	38.012352
2116.045087	225903.565447	38.017370
2118.358195	226232.186846	38.022388
2120.373699	226561.250408	38.027405
2122.510345	226887.286649	38.032423
2124.901393	227201.309588	38.037440
2126.958667	227503.348894	38.042458
2128.853090	227813.211755	38.047476
2130.971882	228124.208389	38.052493
2132.649954	228425.904799	38.057511
2134.797444	228740.200656	38.062528
2136.667888	229062.312957	38.067546
2138.542301	229378.457605	38.072564
2140.519685	229704.187039	38.077581
2142.604612	230035.691103	38.082599
2145.272127	230364.005569	38.087616
2147.276946	230692.527946	38.092634
2149.660036	231018.731178	38.097652
2151.885882	231338.636615	38.102669
2153.935070	231683.511364	38.107687
2156.380312	231999.777891	38.112704
2157.994267	232344.393976	38.117722
2160.308685	232684.709625	38.122740
2162.789792	233025.888985	38.127757
2164.700065	233372.366658	38.132775
2166.954743	233706.904756	38.137792
2168.956791	234050.144789	38.142810
2171.182637	234398.607933	38.147828
2173.359976	234744.057631	38.152845
2175.614305	235106.767121	38.157863
2177.699757	235448.373314	38.162880
2180.127305	235803.387563	38.167898
2182.218471	236146.417521	38.172916
2184.490082	236506.233868	38.177933
2186.477130	236863.937716	38.182951
2188.949748	237212.574620	38.187968
2191.350261	237565.313330	38.192986
2193.395562	237915.874445	38.198004
2196.000479	238274.729623	38.203021
2197.856127	238621.360871	38.208039
2200.030690	238978.610291	38.213056
2202.229779	239339.235079	38.218074
2204.458411	239706.841167	38.223092
2207.039921	240050.466248	38.228109
2208.957890	240412.536034	38.233127
2211.646821	240762.927891	38.238144
2213.976588	241131.386119	38.243162
2215.970036	241479.528266	38.248180
2218.386548	241836.875272	38.253197
2220.246521	242199.289983	38.258215
2222.618314	242544.809848	38.263232
2224.995353	242904.249073	38.268250
2226.977685	243269.517763	38.273268
2229.422381	243627.475151	38.278285
2231.617016	243990.070656	38.283303
2233.665047	244344.409940	38.288320
2236.143976	244704.269949	38.293338
2237.882654	245067.779006	38.298356
2240.467383	245415.711381	38.303373
2242.479299	245780.779293	38.308391
2244.695796	246112.490096	38.313408
2247.409783	246452.911461	38.318426
2249.430368	246780.108218	38.323444
2251.796362	247098.538485	38.328461
2253.707080	247442.188545	38.333479
2256.009072	247774.245355	38.338496
2258.281212	248099.271584	38.343514
2260.291338	248438.234466	38.348532
2262.621277	248774.861310	38.353549
2264.564462	249120.669262	38.358567
2267.169431	249463.096303	38.363584
2269.097970	249808.781130	38.368602
2271.409332	250161.975622	38.373620
2273.830026	250514.061308	38.378637
2275.638546	250879.148782	38.383655
2277.619517	251234.074525	38.388672
2280.451448	251604.386463	38.393690
2282.243631	251975.067301	38.398708
2284.772996	252342.279036	38.403725
2286.843200	252719.877464	38.408743
2289.316073	253088.090401	38.413760
2291.603752	253464.055625	38.418778
2293.780293	253843.976547	38.423796
2296.254266	254213.233077	38.428813
2298.371679	254602.487441	38.433831
2300.700071	254982.462800	38.438848
2303.722001	255369.822560	38.443866
2305.533133	255747.239599	38.448884
2308.080786	256127.995266	38.453901
2310.437872	256503.421981	38.458919
2312.976000	256893.782613	38.463936
2315.149009	257280.899546	38.468954
2317.442160	257664.289371	38.473972
2320.343292	258054.569128	38.478989
2322.456483	258424.703317	38.484007
2324.910232	258813.658162	38.489024
2327.237718	259188.941691	38.494042
2329.700550	259571.139248	38.499060
2331.824883	259967.032268	38.504077
2334.399789	260352.845821	38.509095
2336.472791	260730.026393	38.514112
2339.217585	261104.179677	38.519130
2341.387493	261502.963688	38.524148
2343.829258	261872.644359	38.529165
2346.247456	262270.627997	38.534183
2348.502507	262651.567306	38.539200
2351.016483	263043.592511	38.544218
2353.319172	263424.804649	38.549236
2355.798312	263799.943359	38.554253
2357.939220	264193.883515	38.559271
2360.800382	264573.255621	38.564288
2362.694494	264965.330541	38.569306
2364.798395	265349.446861	38.574324
2367.464830	265727.961918	38.579341
2369.996828	266116.355058	38.584359
2372.295905	266478.035982	38.589376
2374.913602	266819.039337	38.594394
2376.895316	267173.505846	38.599412
2379.243151	267530.099263	38.604429
2381.598246	267893.220420	38.609447
2383.939977	268239.247582	38.614464
2386.284573	268597.214046	38.619482
2388.155407	268965.950618	38.624500
2390.770064	269323.925540	38.629517
2393.112436	269704.171718	38.634535
2395.525598	270073.889928	38.639552
2397.872376	270456.955605	38.644570
2400.174227	270829.587832	38.649588
2402.447984	271211.801751	38.654605
2404.774341	271587.351824	38.659623
2407.193929	271976.376460	38.664640
2409.766292	272358.518117	38.669658
2411.933957	272754.568900	38.674676
2414.339065	273145.171248	38.679693
2416.651113	273547.118369	38.684711
2418.679198	273954.013456	38.689728
2421.080192	274350.434118	38.694746
2423.397481	274768.969082	38.699764
2426.463920	275173.362670	38.704781
2428.454777	275592.635354	38.709799
2431.013902	276009.252239	38.714816
2433.624361	276430.509812	38.719834
2435.762695	276854.204716	38.724852
2438.383043	277265.629546	38.729869
2440.708582	277690.895102	38.734887
2443.156791	278121.882309	38.739904
2445.914237	278537.934016	38.744922
2448.417438	278968.734475	38.749940
2450.708426	279393.624044	38.754957
2453.041090	279822.190345	38.759975
2455.885722	280248.109592	38.764992
2458.509575	280671.116855	38.770010
2460.863388	281104.683692	38.775028
2463.275702	281532.042613	38.780045
2466.138378	281957.196031	38.785063
2468.549872	282382.217467	38.790080
2471.455779	282803.832435	38.795098
2474.022179	283227.050512	38.800116
2476.311498	283645.866620	38.805133
2479.296439	284073.437876	38.810151
2481.482742	284494.987769	38.815168
2484.391184	284913.857127	38.820186
2486.653612	285337.528064	38.825204
2489.370005	285748.653716	38.830221
2492.551279	286163.185516	38.835239
2494.961865	286569.176579	38.840256
2497.646029	286962.015892	38.845274
2500.205764	287357.491021	38.850292
2502.676527	287755.545516	38.855309
2505.039253	288142.617196	38.860327
2507.534363	288527.025547	38.865344
2510.426715	288876.974973	38.870362
2512.461016	289255.079352	38.875380
2514.568107	289629.056473	38.880397
2517.283231	289992.496221	38.885415
2519.437395	290372.053559	38.890432
2521.620742	290742.409974	38.895450
2524.141879	291127.852377	38.900468
2526.402791	291520.016367	38.905485
2528.823764	291906.311805	38.910503
2531.065312	292304.853737	38.915520
2533.613418	292691.559677	38.920538
2536.046202	293098.884710	38.925556
2538.312969	293503.745914	38.930573
2541.212053	293922.629962	38.935591
2543.383621	294335.785976	38.940608
2545.694588	294760.045350	38.945626
2548.160026	295179.452988	38.950644
2550.626651	295610.874861	38.955661
2553.131049	296050.697969	38.960679
2555.803929	296481.323271	38.965696
2558.660937	296915.271538	38.970714
2561.087719	297357.441050	38.975732
2563.615907	297804.013407	38.980749
2566.557361	298239.545609	38.985767
2568.516860	298696.239663	38.990784
2571.342471	299137.630483	38.995802
2574.121300	299581.313762	39.000820
2576.592702	300034.417810	39.005837
2579.341275	300480.415104	39.010855
2581.811524	300936.057061	39.015872
2584.939953	301384.354067	39.020890
2587.490695	301840.615765	39.025908
2589.893627	302291.717707	39.030925
2592.652249	302732.322096	39.035943
2595.291746	303194.255619	39.040960
2597.976333	303642.921239	39.045978
2600.996864	304106.061616	39.050996
2603.745678	304548.795862	39.056013
2606.359684	304998.509913	39.061031
2608.856403	305450.501772	39.066048
2612.035894	305896.821248	39.071066
2614.653020	306346.454229	39.076084
2617.148292	306780.915537	39.081101
2619.877671	307222.425037	39.086119
2622.644652	307677.643245	39.091136
2625.018907	308117.681943	39.096154
2627.852046	308564.047246	39.101172
2630.580835	309003.696487	39.106189
2633.311759	309443.953424	39.111207
2635.660483	309894.886452	39.116224
2638.660923	310341.167994	39.121242
2641.128601	310780.090163	39.126260
2643.895663	311226.557727	39.131277
2646.735052	311641.008803	39.136295
2649.004187	312061.111176	39.141312
2651.639592	312465.533416	39.146330
2654.626230	312866.469666	39.151348
2656.898837	313262.793345	39.156365
2659.460167	313666.613353	39.161383
2661.956485	314079.661955	39.166400
2664.762886	314485.370390	39.171418
2666.944151	314901.030994	39.176436
2669.245153	315332.799093	39.181453
2671.961834	315751.597116	39.186471
2674.484763	316180.964451	39.191488
2677.243600	316619.181999	39.196506
2679.655493	317060.094000	39.201524
2682.372333	317504.003507	39.206541
2685.029285	317938.751842	39.211559
2687.430726	318400.739768	39.216576
2690.273784	318846.172422	39.221594
2693.038943	319304.110938	39.226612
2695.413905	319772.090230	39.231629
2698.362213	320222.096645	39.236647
2700.928570	320691.514025	39.241664
2703.422899	321151.391105	39.246682
2706.445452	321626.090177	39.251700
2708.856594	322101.543886	39.256717
2711.938838	322571.022118	39.261735
2714.186513	323050.534662	39.266752
2717.321552	323530.869069	39.271770
2720.108849	323999.345031	39.276788
2722.670158	324482.126809	39.281805
2726.025687	324969.427483	39.286823
2728.746194	325444.381942	39.291840
2731.465773	325930.838043	39.296858
2734.260420	326406.181526	39.301876
2736.940127	326880.092885	39.306893
2740.439563	327363.775744	39.311911
2743.229005	327851.072618	39.316928
2745.775544	328316.971660	39.321946
2748.825342	328792.641371	39.326964
2751.814342	329280.507179	39.331981
2754.374442	329739.894481	39.336999
2757.225191	330210.457236	39.342016
2759.954986	330683.042337	39.347034
2762.686405	331158.265156	39.352052
2765.629450	331632.486443	39.357069
2768.722797	332097.336011	39.362087
2771.416677	332584.084230	39.367104
2774.207848	333036.710586	39.372122
2777.391132	333506.336156	39.377140
2779.805904	333984.739311	39.382157
2782.903428	334446.932075	39.387175
2786.010410	334921.181765	39.392192
2788.523239	335377.620631	39.397210
2791.251165	335835.977606	39.402228
2793.747585	336303.687055	39.407245
2796.998589	336754.667464	39.412263
2799.548857	337203.521334	39.417280
2801.975416	337626.593922	39.422298
2804.889096	338057.305661	39.427316
2807.460803	338489.566812	39.432333
2810.108063	338926.916743	39.437351
2812.774704	339361.264526	39.442368
2815.519924	339806.134089	39.447386
2818.086265	340250.622631	39.452404
2820.567170	340715.789353	39.457421
2823.591427	341166.064125	39.462439
2826.004084	341624.074890	39.467456
2828.352721	342099.078199	39.472474
2831.424413	342559.110436	39.477492
2834.090305	343040.352860	39.482509
2836.915941	343521.159954	39.487527
2839.787134	343997.487540	39.492544
2842.562779	344487.917258	39.497562
2845.461647	344978.831196	39.502580
2848.066831	345483.700390	39.507597
2851.334145	345976.604130	39.512615
2853.837061	346474.549989	39.517632
2856.828349	346980.411370	39.522650
2859.718252	347486.055860	39.527668
2862.709837	347992.314448	39.532685
2865.501417	348502.585941	39.537703
2868.358557	349011.877723	39.542720
2871.511283	349533.405164	39.547738
2874.619646	350042.165392	39.552756
2877.222417	350553.539575	39.557773
2880.377702	351072.792661	39.562791
2883.454390	351581.695890	39.567808
2886.092002	352109.423624	39.572826
2889.287732	352612.814999	39.577844
2891.810698	353130.422117	39.582861
2895.014075	353646.241060	39.587879
2898.269118	354173.418957	39.592896
2901.156767	354694.633647	39.597914
2904.236263	355208.222941	39.602932
2906.914657	355728.698798	39.607949
2910.115692	356242.410793	39.612967
2912.831057	356773.429600	39.617984
2915.585600	357313.422134	39.623002
2919.140417	357821.097080	39.628020
2922.098047	358361.629931	39.633037
2925.052522	358873.247257	39.638055
2928.075067	359388.275019	39.643072
2930.978169	359910.956087	39.648090
2934.080434	360428.143040	39.653108
2936.826084	360955.431752	39.658125
2939.827201	361468.308772	39.663143
2942.747404	361986.802147	39.668160
2945.744521	362505.962934	39.673178
2949.040510	363011.365578	39.678196
2951.483504	363537.480607	39.683213
2954.386871	364041.208437	39.688231
2957.250526	364535.699112	39.693248
2960.075902	365019.404570	39.698266
2962.961813	365487.893628	39.703284
2965.333522	365978.411403	39.708301
2968.461632	366470.301431	39.713319
2971.436531	366964.595834	39.718336
2974.146628	367462.504900	39.723354
2977.011129	367956.425134	39.728372
2980.248064	368456.751992	39.733389
2982.942396	368964.442104	39.738407
2985.829863	369473.364573	39.743424
2988.667490	370002.158313	39.748442
2991.715940	370511.043143	39.753460
2994.406913	371036.117225	39.758477
2997.282570	371558.339019	39.763495
3000.347954	372091.384737	39.768512
3003.173058	372632.784560	39.773530
3006.477562	373177.755407	39.778548
3009.212743	373714.664321	39.783565
3012.261384	374275.418392	39.788583
3015.256816	374817.295784	39.793600
3018.260829	375377.610614	39.798618
3021.542713	375932.418756	39.803636
3024.408759	376495.251948	39.808653
3027.515003	377047.636945	39.813671
3030.724008	377599.211593	39.818688
3033.353879	378178.727554	39.823706
3037.246384	378739.489402	39.828724
3040.444560	379295.329897	39.833741
3043.526283	379851.028760	39.838759
3046.535639	380427.508778	39.843776
3049.397828	380988.325468	39.848794
3052.806090	381547.829928	39.853812
3055.837792	382125.904746	39.858829
3058.912321	382690.595158	39.863847
3062.355484	383256.537987	39.868864
3065.033800	383830.787012	39.873882
3068.102797	384390.430289	39.878900
3071.041380	384960.384632	39.883917
3074.180321	385534.002012	39.888935
3077.790340	386105.405273	39.893952
3080.624937	386687.854824	39.898970
3084.225064	387248.208041	39.903988
3087.055603	387837.666030	39.909005
3089.922844	388407.350065	39.914023
3093.266830	388970.684869	39.919040
3096.066043	389562.174179	39.924058
3099.199567	390126.183601	39.929076
3102.462233	390704.036912	39.934093
3105.284610	391290.852539	39.939111
3108.380693	391876.220208	39.944128
3111.569910	392470.439782	39.949146
3114.843503	393045.412458	39.954164
3117.660456	393630.236950	39.959181
3120.984609	394195.317383	39.964199
3124.184839	394747.652319	39.969216
3126.895021	395293.310366	39.974234
3129.857075	395839.934172	39.979252
3133.056612	396378.625174	39.984269
3135.749315	396940.412707	39.989287
3138.814071	397499.190524	39.994304
3141.731716	398058.362639	39.999322
3145.218535	398610.639750	40.004340
3147.727118	399186.542223	40.009357
3150.399745	399766.085267	40.014375
3153.562658	400333.496771	40.019392
3156.202688	400942.563018	40.024410
3159.099172	401546.988159	40.029428
3162.470726	402137.940027	40.034445
3165.605271	402770.143118	40.039463
3168.891284	403359.260617	40.044480
3171.766802	403996.551018	40.049498
3175.318797	404618.865411	40.054516
3178.404133	405233.306388	40.059533
3181.426401	405868.152788	40.064551
3184.607852	406498.423409	40.069568
3188.056410	407130.616302	40.074586
3191.151925	407773.422808	40.079604
3194.758478	408402.396023	40.084621
3197.662320	409041.023803	40.089639
3201.286897	409691.919250	40.094656
3204.398105	410341.589254	40.099674
3207.876864	410979.705127	40.104692
3211.157051	411639.636520	40.109709
3214.222305	412290.310901	40.114727
3217.734042	412926.580529	40.119744
3220.726603	413593.534707	40.124762
3223.935491	414239.049377	40.129780
3227.613095	414899.909788	40.134797
3230.591240	415553.947334	40.139815
3234.436736	416213.002778	40.144832
3237.205245	416872.416306	40.149850
3241.157518	417509.327419	40.154868
3244.435699	418173.065173	40.159885
3247.736230	418826.926763	40.164903
3251.247448	419463.585298	40.169920
3254.534737	420124.615407	40.174938
3258.468725	420761.836589	40.179956
3261.708735	421395.631130	40.184973
3264.990449	422041.693104	40.189991
3268.329658	422670.451560	40.195008
3271.571453	423327.055156	40.200026
3275.048169	423954.267805	40.205044
3278.466113	424591.583909	40.210061
3281.289576	425234.603307	40.215079
3285.016645	425859.579194	40.220096
3288.013960	426502.465039	40.225114
3291.127589	427142.505279	40.230132
3294.691916	427775.948748	40.235149
3297.680381	428408.759006	40.240167
3301.011667	429010.090267	40.245184
3303.870147	429604.643594	40.250202
3306.976970	430211.049024	40.255220
3310.178813	430807.344615	40.260237
3313.219999	431414.239195	40.265255
3316.534715	432021.861551	40.270272
3319.302105	432654.528609	40.275290
3322.293107	433275.646695	40.280308
3325.452846	433905.587123	40.285325
3328.614813	434551.745102	40.290343
3331.849106	435187.669572	40.295360
3334.745335	435841.079703	40.300378
3338.170444	436490.844124	40.305396
3341.525932	437157.062432	40.310413
3344.395267	437849.699922	40.315431
3348.145771	438512.451981	40.320448
3351.557972	439182.354949	40.325466
3354.715756	439862.914351	40.330484
3358.144589	440545.589593	40.335501
3361.606017	441248.748566	40.340519
3364.656359	441942.382336	40.345536
3367.916552	442651.102681	40.350554
3371.184939	443350.687271	40.355572
3374.953883	444055.235562	40.360589
3377.805433	444784.868510	40.365607
3381.146606	445490.809363	40.370624
3384.714391	446229.853655	40.375642
3387.917761	446967.717616	40.380660
3391.843327	447687.068254	40.385677
3395.043760	448427.165143	40.390695
3398.768443	449158.449203	40.395712
3402.019603	449892.974204	40.400730
3405.564287	450628.391335	40.405748
3409.145859	451366.512508	40.410765
3412.756461	452111.083996	40.415783
3416.739415	452838.971828	40.420800
3420.240615	453570.556600	40.425818
3423.570926	454319.908490	40.430836
3426.756677	455062.831421	40.435853
3430.502209	455800.479694	40.440871
3434.175152	456544.592506	40.445888
3437.487294	457277.453435	40.450906
3440.861831	458008.307021	40.455924
3444.848990	458749.463008	40.460941
3448.264557	459505.205810	40.465959
3451.773432	460230.348525	40.470976
3455.510865	460960.085742	40.475994
3459.006453	461699.398661	40.481012
3462.350152	462413.162532	40.486029
3465.533383	463178.477764	40.491047
3469.527997	463868.718941	40.496064
3472.668899	464638.744159	40.501082
3475.772776	465343.040146	40.506100
3479.828671	466100.626954	40.511117
3483.174221	466822.524920	40.516122
3486.554497	467497.322165	40.521127
3489.917610	468111.912727	40.526132
3492.951825	468677.201865	40.531136
3495.739784	469178.882122	40.536141
3498.272486	469643.172507	40.541146
3501.223252	470037.672397	40.546151
3503.492815	470383.904373	40.551156
3505.851942	470661.317030	40.556160
3508.438764	470880.639512	40.561165
3509.848419	471072.413574	40.566170
3511.610236	471200.301018	40.571175
3513.411857	471284.935876	40.576180
3514.223247	471345.543963	40.581184
3515.402287	471363.558191	40.586189
3516.635437	471351.297157	40.591194
3517.636724	471313.977217	40.596199
3518.476607	471241.295351	40.601204
3519.095131	471140.865443	40.606208
3519.979558	471026.552249	40.611213
3520.125378	470891.467139	40.616218
3520.432308	470738.610862	40.621223
3520.605111	470574.620684	40.626228
3520.878529	470399.408535	40.631232
3520.965785	470197.961323	40.636237
3521.013737	469993.019984	40.641242
3521.492787	469798.148851	40.646247
3521.960022	469583.351762	40.651252
3521.679082	469355.335875	40.656256
3521.695585	469105.366592	40.661261
3521.653867	468872.997840	40.666266
3521.480337	468639.227619	40.671271
3521.552329	468393.449561	40.676276
3521.047604	468163.427875	40.681280
3520.941011	467916.506239	40.686285
3520.384425	467676.802518	40.691290
3520.453340	467428.123385	40.696295
3520.499590	467187.304667	40.701300
3519.811849	466947.106314	40.706304
3519.655175	466706.719873	40.711309
3519.344224	466478.170480	40.716314
3519.081309	466255.645565	40.721319
3519.259975	466022.247103	40.726324
3518.677839	465790.386263	40.731328
3518.431662	465558.266946	40.736333
3517.969029	465336.372538	40.741338
3518.021933	465106.280246	40.746343
3517.665347	464881.321567	40.751348
3517.212865	464676.204899	40.756352
3517.234337	464454.021962	40.761357
3516.818916	464252.648266	40.766362
3516.259785	464046.477420	40.771367
3515.783733	463854.390524	40.776372
3515.619279	463661.745494	40.781376
3515.396794	463475.701116	40.786381
3514.906330	463294.109903	40.791386
3514.849432	463103.674452	40.796391
3514.606885	462929.750091	40.801396
3514.454629	462771.583539	40.806400
3514.388017	462593.976933	40.811405
3514.078729	462437.962966	40.816410
3513.787120	462263.990297	40.821415
3513.601269	462099.991386	40.826420
3513.231062	461945.505114	40.831424
3513.031377	461791.751603	40.836429
3512.791541	461652.813942	40.841434
3512.583341	461502.508776	40.846439
3512.984176	461352.968574	40.851444
3512.135372	461232.080030	40.856448
3511.933393	461074.872721	40.861453
3512.216378	460936.202913	40.866458
3512.014965	460810.289584	40.871463
3511.812400	460676.665751	40.876468
3511.538017	460542.798837	40.881472
3511.666537	460415.005028	40.886477
3511.258742	460305.505284	40.891482
3511.014566	460173.153068	40.896487
3511.117423	460045.158265	40.901492
3510.301937	459934.960244	40.906496
3510.195316	459818.613293	40.911501
3510.297293	459712.124262	40.916506
3510.297559	459605.295713	40.921511
3509.975144	459516.474706	40.926516
3509.863010	459414.786338	40.931520
3510.102292	459297.570338	40.936525
3509.431112	459202.614550	40.941530
3509.341918	459109.037440	40.946535
3509.455196	459020.094838	40.951540
3509.176930	458934.358873	40.956544
3508.984655	458838.108356	40.961549
3508.911882	458746.759137	40.966554
3508.571391	458655.705500	40.971559
3508.968092	458585.536465	40.976564
3508.660845	458505.890812	40.981568
3508.540897	458407.851498	40.986573
3508.028038	458344.724576	40.991578
3508.077720	458268.927769	40.996583
3508.411051	458192.020553	41.001588
3508.319338	458118.021102	41.006592
3508.117452	458046.423106	41.011597
3508.037571	457981.603365	41.016602
3508.070683	457900.024740	41.021607
3507.679571	457833.985522	41.026612
3507.639131	457787.573954	41.031616
3507.680891	457703.608928	41.036621
3507.886803	457650.816849	41.041626
3507.539668	457588.118154	41.046631
3507.369516	457522.651850	41.051636
3507.220723	457468.951527	41.056640
3507.257756	457402.234580	41.061645
3507.346335	457352.605661	41.066650
3507.021016	457287.112463	41.071655
3506.961893	457234.970070	41.076660
3506.839390	457183.040499	41.081664
3507.217683	457120.580939	41.086669
3506.751065	457075.655742	41.091674
3506.482320	457022.785015	41.096679
3507.046816	456982.668355	41.101684
3506.694752	456934.376460	41.106688
3506.444147	456890.583581	41.111693
3506.236010	456827.201259	41.116698
3506.282568	456785.136829	41.121703
3506.465020	456759.691076	41.126708
3506.303014	456714.666269	41.131712
3506.501573	456664.815509	41.136717
3506.260493	456636.849202	41.141722
3506.292010	456593.619938	41.146727
3506.269078	456539.593090	41.151732
3506.169129	456508.966202	41.156736
3506.157462	456476.955525	41.161741
3506.260780	456433.359471	41.166746
3505.993573	456379.421584	41.171751
3505.984775	456349.997669	41.176756
3505.944004	456329.304914	41.181760
3506.080702	456274.846328	41.186765
3505.996808	456245.738549	41.191770
3505.721735	456215.697013	41.196775
3506.068046	456172.062040	41.201780
3505.478347	456146.585448	41.206784
3505.478380	456106.302783	41.211789
3505.512536	456069.160157	41.216794
3505.730969	456031.430267	41.221799
3505.723300	456002.817463	41.226804
3505.643761	455983.500339	41.231808
3505.786471	455928.126748	41.236813
3505.175179	455908.893617	41.241818
3505.478156	455880.485224	41.246823
3505.461184	455855.881722	41.251828
3505.414206	455835.138758	41.256832
3505.388237	455796.432418	41.261837
3505.255206	455773.064801	41.266842
3505.339910	455756.410455	41.271847
3505.581277	455735.621819	41.276852
3505.276563	455710.150418	41.281856
3505.447456	455678.261950	41.286861
3505.105507	455645.541275	41.291866
3504.822560	455621.131766	41.296871
3505.602757	455598.989454	41.301876
3505.244343	455579.868271	41.306880
3505.452475	455541.986984	41.311885
3505.409548	455519.518094	41.316890
3505.458601	455490.692734	41.321895
3505.685252	455466.354707	41.326900
3505.118407	455445.338415	41.331904
3505.244062	455434.714868	41.336909
3505.142527	455405.862467	41.341914
3504.848877	455377.497018	41.346919
3504.931658	455358.711790	41.351924
3505.077829	455332.762803	41.356928
3504.994948	455317.250808	41.361933
3504.711482	455306.235251	41.366938
3505.004754	455278.030577	41.371943
3505.061888	455255.241192	41.376948
3504.595121	455246.486956	41.381952
3504.895720	455217.266332	41.386957
3504.793470	455200.844073	41.391962
3504.620331	455194.123574	41.396967
3504.734479	455185.176014	41.401972
3504.622384	455158.455877	41.406976
3504.766675	455153.004324	41.411981
3504.706887	455127.087658	41.416986
3504.398932	455126.070892	41.421991
3504.889325	455097.987043	41.426996
3504.604898	455085.906070	41.432000
3504.721883	455070.768201	41.437005
3504.790317	455052.289403	41.442010
3504.555355	455044.056545	41.447015
3504.843955	455014.736083	41.452020
3504.635348	455012.587408	41.457024
3504.547877	454992.053015	41.462029
3504.508717	454980.897207	41.467034
3504.367073	454968.692129	41.472039
3504.927009	454955.006256	41.477044
3504.642145	454952.413000	41.482048
3504.708804	454936.623422	41.487053
3505.034444	454929.976210	41.492058
3504.346282	454903.042414	41.497063
3504.315834	454877.425243	41.502068
3504.507728	454879.272177	41.507072
3504.390725	454860.619590	41.512077
3504.395623	454860.872510	41.517082
3504.268977	454868.807464	41.522087
3504.458884	454822.607037	41.527092
3504.425497	454828.548528	41.532096
3504.419580	454819.974960	41.537101
3504.449800	454805.814628	41.542106
3504.330552	454794.975810	41.547111
3504.674361	454785.382946	41.552116
3504.514194	454772.876268	41.557120
3504.528301	454763.589198	41.562125
3504.548604	454744.914810	41.567130
3504.475528	454729.045702	41.572135
3504.941506	454717.150333	41.577140
3504.493252	454699.260294	41.582144
3504.814541	454685.967143	41.587149
3504.629630	454668.086188	41.592154
3504.500185	454664.504325	41.597159
3504.290162	454646.221425	41.602164
3504.202355	454635.022400	41.607168
3504.444091	454621.234414	41.612173
3504.305097	454624.554317	41.617178
3504.248558	454614.517294	41.622183
3504.696949	454588.925579	41.627188
3504.505903	454611.229454	41.632192
3503.947893	454588.181476	41.637197
3504.791872	454567.093560	41.642202
3504.899095	454554.138595	41.647207
3504.714312	454546.151309	41.652212
3504.399094	454542.903218	41.657216
3504.825722	454511.835217	41.662221
3504.860337	454501.732997	41.667226
3504.724014	454494.702046	41.672231
3504.996246	454475.683187	41.677236
3504.214801	454452.670391	41.682240
3504.470275	454428.783332	41.687245
3504.688473	454428.596639	41.692250
3504.588978	454397.916075	41.697255
3504.543456	454391.986968	41.702260
3504.094718	454383.026595	41.707264
3504.306202	454359.603057	41.712269
3504.424744	454354.713499	41.717274
3504.135444	454367.037792	41.722279
3504.714890	454339.547781	41.727284
3504.538771	454337.343167	41.732288
3504.314309	454325.810425	41.737293
3504.120490	454309.452732	41.742298
3504.115555	454313.258867	41.747303
3504.056386	454299.010873	41.752308
3504.222562	454310.197700	41.757312
3504.206630	454284.019447	41.762317
3504.164288	454277.683904	41.767322
3503.699509	454281.055355	41.772327
3504.265513	454276.450214	41.777332
3504.226071	454281.479521	41.782336
3504.108210	454257.194655	41.787341
3504.361601	454258.524539	41.792346
3504.540614	454247.739786	41.797351
3504.540441	454238.657710	41.802356
3504.340146	454239.044550	41.807360
3504.541081	454215.216627	41.812365
3504.731469	454194.130207	41.817370
3504.317111	454211.243741	41.822375
3504.235654	454185.380162	41.827380
3504.172803	454167.885422	41.832384
3504.261668	454167.617695	41.837389
3504.260314	454158.434298	41.842394
3503.965162	454148.739217	41.847399
3504.175125	454126.990044	41.852404
3504.300572	454138.741515	41.857408
3504.424869	454142.780942	41.862413
3504.428392	454116.751636	41.867418
3504.183502	454115.369685	41.872423
3504.219453	454116.480257	41.877428
3504.380956	454110.163182	41.882432
3504.343630	454089.924476	41.887437
3504.085673	454076.824012	41.892442
3504.402869	454070.989699	41.897447
3504.662808	454054.204924	41.902452
3504.156343	454039.418612	41.907456
3504.118998	454057.030789	41.912461
3504.728627	454039.277432	41.917466
3504.233556	454017.944034	41.922471
3504.335941	454016.101272	41.927476
3504.431214	453982.801692	41.932480
3504.261221	453984.553690	41.937485
3504.236917	453987.449646	41.942490
3504.201051	453964.369233	41.947495
3504.722549	453948.405592	41.952500
3504.047455	453946.432031	41.957504
3504.404273	453941.707674	41.962509
3504.390797	453925.676368	41.967514
3504.382436	453916.392502	41.972519
3504.329523	453902.752137	41.977524
3504.308661	453894.129843	41.982528
3504.526479	453880.649624	41.987533
3504.430592	453879.802232	41.992538
3504.259392	453871.406650	41.997543
3504.534992	453858.627628	42.002548
3504.283181	453860.798480	42.007552
3503.931790	453843.653536	42.012557
3504.194875	453842.901615	42.017562
3503.725482	453843.178782	42.022567
3504.325210	453841.054432	42.027572
3504.344563	453835.165663	42.032576
3504.334700	453810.508076	42.037581
3504.317591	453803.762499	42.042586
3504.171264	453801.806818	42.047591
3504.395468	453781.171322	42.052596
3504.397641	453780.511382	42.057600
3504.289827	453778.194438	42.062605
3504.518275	453753.651334	42.067610
3504.002708	453746.984535	42.072615
3504.164839	453749.800311	42.077620
3503.839392	453753.860163	42.082624
3503.861059	453731.227071	42.087629
3504.062755	453720.742919	42.092634
3503.873666	453724.324568	42.097639
3504.372821	453713.844130	42.102644
3504.037338	453726.176069	42.107648
3503.946930	453716.397700	42.112653
3504.338312	453687.668151	42.117658
3504.238714	453686.770599	42.122663
3504.369153	453686.547034	42.127668
3504.123486	453675.626186	42.132672
3504.214226	453656.127940	42.137677
3504.224484	453660.236219	42.142682
3504.026343	453659.252765	42.147687
3504.324755	453647.839982	42.152692
3504.334157	453637.487668	42.157696
3504.099235	453632.349393	42.162701
3504.160418	453633.050085	42.167706
3503.971718	453630.999609	42.172711
3504.165098	453598.445050	42.177716
3504.277944	453606.596283	42.182720
3504.205000	453599.352077	42.187725
3504.260690	453596.400394	42.192730
3504.274901	453573.717585	42.197735
3504.523008	453572.968023	42.202740
3504.224778	453559.112533	42.207744
3504.259519	453542.515198	42.212749
3504.231541	453532.067266	42.217754
3504.310619	453535.910991	42.222759
3504.473795	453515.081943	42.227764
3504.443064	453498.089009	42.232768
3504.437972	453499.612017	42.237773
3504.496223	453468.194907	42.242778
3503.669513	453466.498969	42.247783
3504.253645	453464.681490	42.252788
3504.114704	453471.705557	42.257792
3503.712610	453457.003846	42.262797
3503.884528	453451.293821	42.267802
3503.882464	453432.469672	42.272807
3503.845797	453434.555814	42.277812
3504.105761	453444.206045	42.282816
3504.184474	453451.753851	42.287821
3504.503828	453426.891588	42.292826
3504.296537	453412.666453	42.297831
3504.426272	453397.119536	42.302836
3504.449452	453403.712076	42.307840
3504.292396	453387.753828	42.312845
3504.703638	453386.927732	42.317850
3504.291863	453370.502336	42.322855
3504.324106	453362.734027	42.327860
3504.446315	453356.067775	42.332864
3504.383346	453339.384259	42.337869
3504.913270	453321.998127	42.342874
3504.325416	453329.042460	42.347879
3504.315184	453292.967844	42.352884
3504.143359	453282.999198	42.357888
3504.379931	453278.293714	42.362893
3504.529053	453267.411743	42.367898
3504.303456	453248.774999	42.372903
3504.017416	453241.665845	42.377908
3504.199206	453247.472254	42.382912
3504.080198	453223.034245	42.387917
3504.352915	453223.447810	42.392922
3503.999649	453225.533278	42.397927
3504.342184	453213.453680	42.402932
3503.939578	453197.635595	42.407936
3504.002844	453189.507140	42.412941
3504.111939	453186.952885	42.417946
3503.979284	453186.973866	42.422951
3504.100980	453188.020190	42.427956
3503.917232	453163.338649	42.432960
3503.923157	453152.580741	42.437965
3504.331341	453154.495108	42.442970
3504.003320	453161.193975	42.447975
3504.291337	453156.074410	42.452980
3504.043974	453145.204315	42.457984
3504.318948	453126.437602	42.462989
3504.419008	453127.487348	42.467994
3504.108267	453116.830221	42.472999
3504.339487	453098.171882	42.478004
3504.125329	453098.763894	42.483008
3504.215658	453094.385933	42.488013
3504.449344	453083.338285	42.493018
3504.178153	453075.161179	42.498023
3504.234507	453056.073782	42.503028
3504.021096	453069.401591	42.508032
3504.250921	453045.923065	42.513037
3504.393892	453021.037503	42.518042
3503.896281	453027.509513	42.523047
3504.145715	453015.292306	42.528052
3504.281739	453000.302273	42.533056
3504.034806	452990.040927	42.538061
3504.169180	452987.634876	42.543066
3503.865560	452998.338462	42.548071
3503.990860	453000.855709	42.553076
3504.173520	452976.978641	42.558080
3504.099597	452969.328462	42.563085
3504.213209	452956.777508	42.568090
3503.937897	452963.671064	42.573095
3504.009653	452967.262338	42.578100
3503.924701	452958.040931	42.583104
3504.072344	452934.270836	42.588109
3504.343923	452915.605969	42.593114
3503.637501	452940.935924	42.598119
3503.824529	452939.434883	42.603124
3503.788171	452935.381364	42.608128
3503.914980	452914.811223	42.613133
3504.307190	452899.323958	42.618138
3503.881455	452907.205390	42.623143
3504.277079	452895.370938	42.628148
3504.310484	452900.338293	42.633152
3503.852440	452889.095452	42.638157
3504.280167	452881.568910	42.643162
3503.802955	452885.500680	42.648167
3503.924381	452874.978089	42.653172
3504.073814	452877.491534	42.658176
3503.831172	452863.880540	42.663181
3503.879935	452849.360872	42.668186
3503.729265	452851.465089	42.673191
3504.058476	452849.484896	42.678196
3504.152046	452850.281975	42.683200
3503.749847	452853.390035	42.688205
3503.941469	452843.668191	42.693210
3503.763528	452836.034411	42.698215
3503.893239	452818.000785	42.703220
3503.704833	452813.616091	42.708224
3504.146968	452823.339270	42.713229
3504.144170	452829.580894	42.718234
3503.990554	452843.711242	42.723239
3504.255755	452817.689831	42.728244
3504.035978	452804.734823	42.733248
3503.858921	452812.779942	42.738253
3504.482331	452794.313066	42.743258
3503.857139	452799.942706	42.748263
3504.010387	452777.135647	42.753268
3504.224150	452774.209611	42.758272
3503.869914	452761.377316	42.763277
3504.236892	452762.689334	42.768282
3504.023720	452762.418594	42.773287
3504.411216	452727.599491	42.778292
3504.453569	452734.138453	42.783296
3504.098523	452740.182076	42.788301
3504.144637	452710.135862	42.793306
3504.128237	452701.055739	42.798311
3504.183202	452687.854268	42.803316
3504.205791	452688.408866	42.808321
3504.093852	452681.627207	42.813325
3504.124149	452669.241489	42.818330
3503.861890	452670.855947	42.823335
3504.201039	452668.316010	42.828340
3504.196743	452662.329194	42.833345
3503.865608	452645.383113	42.838349
3504.139237	452629.914412	42.843354
3503.948807	452627.965601	42.848359
3504.174801	452633.612954	42.853364
3504.321157	452639.526602	42.858369
3504.033567	452620.899145	42.863373
3503.893978	452607.474674	42.868378
3503.838135	452606.468679	42.873383
3504.126302	452592.925839	42.878388
3504.179874	452598.854165	42.883393
3503.518538	452591.804134	42.888397
3503.839240	452574.349026	42.893402
3504.307048	452569.759069	42.898407
3504.221152	452567.641504	42.903412
3503.842394	452564.859847	42.908417
3504.147425	452578.714890	42.913421
3504.370516	452553.460962	42.918426
3503.703724	452541.439078	42.923431
3503.836740	452525.332890	42.928436
3504.035706	452551.129056	42.933441
3504.025014	452550.420372	42.938445
3504.402181	452526.207638	42.943450
3504.310690	452508.614670	42.948455
3504.233329	452515.629296	42.953460
3504.187568	452511.323478	42.958465
3503.961670	452481.167737	42.963469
3504.068763	452471.560582	42.968474
3503.723264	452479.530961	42.973479
3504.165801	452472.255654	42.978484
3503.997021	452454.522637	42.983489
3503.613262	452466.253979	42.988493
3504.021821	452453.097962	42.993498
3504.034240	452445.738413	42.998503
3503.860457	452430.543271	43.003508
3503.908781	452441.901870	43.008513
3503.984323	452451.733901	43.013517
3504.026970	452435.134514	43.018522
3503.921439	452444.487750	43.023527
3504.088685	452404.882477	43.028532
3503.707702	452409.255796	43.033537
3503.840820	452416.947570	43.038541
3503.809131	452390.059247	43.043546
3503.759065	452421.273597	43.048551
3503.976169	452395.005599	43.053556
3503.844262	452419.737888	43.058561
3503.854673	452394.618890	43.063565
3503.930175	452410.184810	43.068570
3503.700467	452392.106181	43.073575
3503.879264	452409.381006	43.078580
3503.825957	452402.640738	43.083585
3503.803745	452386.609733	43.088589
3503.856754	452404.107416	43.093594
3504.059240	452399.356398	43.098599
3503.833697	452384.423118	43.103604
3504.139818	452395.994700	43.108609
3503.658379	452371.663817	43.113613
3503.998727	452372.980068	43.118618
3503.930018	452376.339927	43.123623
3504.008268	452366.940257	43.128628
3503.769032	452367.079571	43.133633
3504.109831	452335.565501	43.138637
3503.684749	452338.677246	43.143642
3504.459054	452329.218273	43.148647
3504.271917	452348.124002	43.153652
3504.130110	452331.756668	43.158657
3503.926285	452312.912750	43.163661
3504.356348	452295.541628	43.168666
3503.889748	452317.434618	43.173671
3504.157957	452304.503672	43.178676
3504.439763	452279.798329	43.183681
3503.937696	452273.484158	43.188685
3504.188528	452269.232896	43.193690
3504.178253	452264.109543	43.198695
3504.318339	452256.831236	43.203700
3503.948844	452243.798093	43.208705
3503.817542	452234.837434	43.213709
3504.389890	452252.760562	43.218714
3504.027207	452218.059273	43.223719
3504.353265	452234.093130	43.228724
3504.381022	452195.930339	43.233729
3503.913126	452217.265460	43.238733
3503.827361	452167.043831	43.243738
3503.991425	452193.404086	43.248743
3504.184740	452168.509641	43.253748
3504.239100	452148.660664	43.258753
3504.042581	452178.629926	43.263757
3504.199900	452137.046798	43.268762
3504.012390	452157.779482	43.273767
3503.776872	452123.920574	43.278772
3504.211477	452139.379169	43.283777
3504.204038	452136.893962	43.288781
3503.962763	452098.519822	43.293786
3503.899229	452114.209406	43.298791
3504.115336	452095.755614	43.303796
3504.112569	452094.386007	43.308801
3504.055869	452095.308352	43.313805
3504.219581	452085.641343	43.318810
3503.986281	452071.115029	43.323815
3503.700692	452063.954694	43.328820
3504.042383	452066.387094	43.333825
3504.066661	452076.988532	43.338829
3504.057648	452060.498527	43.343834
3504.196417	452057.736485	43.348839
3504.127895	452031.817681	43.353844
3504.144857	452024.508021	43.358849
3503.788958	452028.065558	43.363853
3504.231350	452023.530255	43.368858
3503.946491	452008.961308	43.373863
3504.069559	451991.537000	43.378868
3504.322443	451986.067528	43.383873
3503.868038	451997.049130	43.388877
3504.035389	451988.802311	43.393882
3504.189566	451974.671372	43.398887
3504.082833	451960.632411	43.403892
3503.967773	451976.228748	43.408897
3504.003418	451974.650089	43.413901
3504.192314	451952.039548	43.418906
3504.227552	451940.363061	43.423911
3503.984782	451942.075974	43.428916
3504.136332	451931.294473	43.433921
3504.109344	451923.129094	43.438925
3504.306265	451899.705342	43.443930
3503.878641	451897.844706	43.448935
3504.209854	451886.527352	43.453940
3504.268457	451891.135739	43.458945
3503.987521	451885.750627	43.463949
3504.178462	451867.605090	43.468954
3504.029091	451861.438026	43.473959
3503.707979	451868.389893	43.478964
3503.856070	451889.323484	43.483969
3503.922425	451870.842440	43.488973
3504.010849	451839.722790	43.493978
3503.920362	451853.387076	43.498983
3503.649272	451837.496517	43.503988
3504.193676	451839.135747	43.508993
3503.910189	451838.876110	43.513997
3504.030108	451830.636733	43.519002
3503.766768	451820.022251	43.524007
3503.611845	451800.206057	43.529012
3503.619292	451816.138341	43.534017
3504.020485	451805.317319	43.539021
3504.144050	451804.790363	43.544026
3503.992441	451812.730322	43.549031
3503.822055	451809.408199	43.554036
3504.085984	451809.265002	43.559041
3503.870196	451797.831098	43.564045
3504.134616	451775.512906	43.569050
3504.042413	451773.497751	43.574055
3503.810583	451781.957837	43.579060
3503.880189	451778.090337	43.584065
3504.030169	451772.840055	43.589069
3504.211896	451765.504268	43.594074
3503.889922	451759.262973	43.599079
3503.849739	451766.677898	43.604084
3503.980831	451752.854934	43.609089
3503.829255	451748.768675	43.614093
3504.091701	451748.980918	43.619098
3503.895235	451737.899135	43.624103
3504.106611	451720.308431	43.629108
3503.989469	451728.344458	43.634113
3503.874591	451715.930432	43.639117
3504.072720	451738.581535	43.644122
3504.077444	451704.430316	43.649127
3503.774587	451707.675055	43.654132
3504.136397	451670.168997	43.659137
3503.850989	451708.119694	43.664141
3504.130937	451685.595986	43.669146
3503.930532	451681.111483	43.674151
3503.779615	451694.937648	43.679156
3504.290424	451662.380908	43.684161
3504.092374	451651.806772	43.689165
3504.113729	451636.580258	43.694170
3503.993754	451649.538913	43.699175
3503.634922	451646.195811	43.704180
3504.404468	451619.991833	43.709185
3504.205140	451624.590303	43.714189
3504.361513	451622.891048	43.719194
3503.943246	451616.309729	43.724199
3503.793296	451597.152244	43.729204
3503.847964	451587.553008	43.734209
3503.674372	451590.980306	43.739213
3503.809599	451595.475152	43.744218
3503.939618	451599.666357	43.749223
3503.797585	451589.945984	43.754228
3503.889491	451586.328647	43.759233
3503.867575	451599.474804	43.764237
3504.016947	451568.040689	43.769242
3503.927279	451564.705771	43.774247
3504.146742	451547.468866	43.779252
3503.904056	451557.250095	43.784257
3503.794849	451562.088051	43.789261
3504.376441	451549.614584	43.794266
3504.159837	451534.374875	43.799271
3503.956650	451526.541673	43.804276
3504.327450	451516.384993	43.809281
3503.798666	451524.080209	43.814285
3503.874885	451522.799570	43.819290
3504.332683	451499.334173	43.824295
3504.122200	451484.905370	43.829300
3503.959053	451485.743078	43.834305
3503.382020	451494.054861	43.839309
3504.146322	451483.988196	43.844314
3503.959394	451480.516407	43.849319
3504.074707	451471.059769	43.854324
3504.042250	451457.313226	43.859329
3504.068955	451460.455158	43.864333
3503.774170	451455.884043	43.869338
3503.662500	451460.671665	43.874343
3503.862120	451444.503449	43.879348
3504.154756	451436.794816	43.884353
3503.889340	451429.326627	43.889357
3503.834855	451418.070014	43.894362
3503.579284	451416.486606	43.899367
3503.740613	451423.666810	43.904372
3504.321638	451415.202161	43.909377
3503.992065	451411.651422	43.914381
3504.075014	451392.609185	43.919386
3503.668377	451391.100400	43.924391
3503.993520	451378.261425	43.929396
3504.029315	451384.649574	43.934401
3503.655128	451391.965184	43.939405
3504.229355	451389.387948	43.944410
3504.049537	451377.034750	43.949415
3503.901051	451370.156992	43.954420
3504.151552	451353.168758	43.959425
3504.003145	451355.627964	43.964429
3504.024021	451355.624675	43.969434
3503.783720	451344.143676	43.974439
3503.694658	451331.065684	43.979444
3504.210457	451319.312917	43.984449
3503.917040	451325.905356	43.989453
3503.978233	451324.068891	43.994458
3504.305856	451331.425814	43.999463
3504.058302	451310.761185	44.004468
3504.211665	451288.409335	44.009473
3503.919105	451293.073352	44.014477
3504.083072	451289.952024	44.019482
3503.906249	451302.057201	44.024487
3503.987119	451266.624682	44.029492
3504.284990	451248.461756	44.034497
3503.789966	451254.172680	44.039501
3503.955370	451245.722926	44.044506
3504.195733	451241.574620	44.049511
3503.879961	451241.066356	44.054516
3504.030451	451224.956497	44.059521
3503.909070	451223.656332	44.064525
3503.818988	451215.906635	44.069530
3503.626594	451226.390480	44.074535
3503.882067	451226.451597	44.079540
3504.035301	451215.009814	44.084545
3503.700665	451220.390925	44.089549
3503.985844	451200.656880	44.094554
3504.139778	451196.978932	44.099559
3503.704494	451184.666014	44.104564
3504.112348	451184.550808	44.109569
3503.795988	451197.540760	44.114573
3504.019905	451189.944397	44.119578
3503.545098	451180.783903	44.124583
3503.567721	451164.897195	44.129588
3503.996927	451157.014646	44.134593
3503.796664	451158.619406	44.139597
3504.132567	451159.733452	44.144602
3504.099469	451160.195399	44.149607
3503.732648	451165.175651	44.154612
3503.826640	451160.289295	44.159617
3503.777989	451162.884987	44.164621
3503.991431	451144.684581	44.169626
3503.978496	451130.985502	44.174631
3503.939482	451117.087558	44.179636
3504.185611	451114.917372	44.184641
3503.696167	451139.910533	44.189645
3503.814384	451128.575733	44.194650
3503.911757	451134.954216	44.199655
3504.118747	451119.596527	44.204660
3503.987012	451106.880369	44.209665
3503.386337	451097.435269	44.214669
3503.491128	451088.792058	44.219674
3503.349899	451106.219941	44.224679
3503.348354	451111.193208	44.229684
3503.808102	451110.613094	44.234689
3503.609040	451111.659472	44.239693
3504.084247	451107.829234	44.244698
3503.816771	451111.677403	44.249703
3503.879482	451116.995726	44.254708
3503.741480	451110.623683	44.259713
3503.746704	451108.491578	44.264717
3503.839914	451083.358062	44.269722
3503.620653	451079.079403	44.274727
3503.369964	451084.599510	44.279732
3503.810483	451069.661578	44.284737
3503.710267	451073.483313	44.289741
3503.671672	451079.122130	44.294746
3503.661010	451075.216456	44.299751
3503.763539	451082.609040	44.304756
3503.707227	451082.313483	44.309761
3503.440601	451094.331475	44.314765
3503.790681	451087.831526	44.319770
3504.176130	451088.886998	44.324775
3503.953679	451083.137237	44.329780
3504.206398	451057.115812	44.334785
3504.194320	451053.464084	44.339789
3503.945796	451046.246827	44.344794
3503.962542	451055.023100	44.349799
3503.750441	451049.982126	44.354804
3503.690541	451028.018952	44.359809
3503.416884	451025.474218	44.364813
3503.576302	451011.595588	44.369818
3503.595848	451015.499891	44.374823
3503.713407	451010.203817	44.379828
3503.880176	451009.771504	44.384833
3503.493811	451024.193485	44.389837
3503.743929	451019.130184	44.394842
3503.920707	451021.182805	44.399847
3503.878131	451019.616445	44.404852
3503.922351	451028.997327	44.409857
3503.814026	451029.978621	44.414861
3503.876141	451018.551145	44.419866
3503.739492	450998.782119	44.424871
3503.803021	451003.491396	44.429876
3504.008595	450988.387570	44.434881
3504.016783	450989.959391	44.439885
3504.097799	450999.689685	44.444890
3503.787844	450997.302921	44.449895
3504.059327	451001.471873	44.454900
3503.896955	450975.921935	44.459905
3503.737011	450971.278662	44.464909
3503.929466	450957.141051	44.469914
3504.076235	450955.494011	44.474919
3503.803665	450963.910090	44.479924
3504.065973	450961.179134	44.484929
3503.602872	450954.452476	44.489933
3503.914970	450936.794510	44.494938
3503.897006	450931.976549	44.499943
3503.827366	450931.074152	44.504948
3504.341713	450924.040736	44.509953
3504.031070	450930.889738	44.514957
3504.148509	450930.820440	44.519962
3504.211876	450906.148158	44.524967
3503.899292	450899.549927	44.529972
3504.009094	450894.661016	44.534977
3504.098423	450890.536522	44.539981
3504.051856	450884.302200	44.544986
3503.910757	450881.990222	44.549991
3503.917317	450879.096703	44.554996
3504.042250	450861.366775	44.560001
3503.578024	450873.365371	44.565005
3504.221772	450869.457707	44.570010
3504.245399	450856.463124	44.575015
3503.867576	450841.552915	44.580020
3504.350228	450828.333518	44.585025
3504.012669	450836.252460	44.590029
3504.101135	450823.349100	44.595034
3503.805354	450810.201999	44.600039
3503.651878	450786.934001	44.605044
3503.869673	450790.502529	44.610049
3503.764874	450788.032568	44.615053
3503.836592	450788.528699	44.620058
3504.003404	450785.508345	44.625063
3503.642762	450793.735424	44.630068
3504.040920	450800.117199	44.635073
3503.239677	450804.607997	44.640077
3503.879661	450796.945735	44.645082
3503.948359	450803.278098	44.650087
3503.820909	450776.504523	44.655092
3503.874078	450759.090336	44.660097
3503.572789	450758.072313	44.665101
3503.564507	450770.100380	44.670106
3504.116360	450768.643021	44.675111
3503.919593	450746.041520	44.680116
3503.778845	450767.782973	44.685121
3504.096687	450761.592504	44.690125
3503.874887	450743.511331	44.695130
3503.761685	450740.535234	44.700135
3503.643661	450728.476396	44.705140
3504.256477	450722.898984	44.710145
3503.885420	450738.079910	44.715149
3503.953961	450742.128752	44.720154
3504.017492	450730.447181	44.725159
3503.634178	450719.445191	44.730164
3503.849875	450707.282842	44.735169
3503.675772	450697.617909	44.740173
3503.494249	450707.389827	44.745178
3503.701707	450703.297373	44.750183
3503.713375	450708.420875	44.755188
3503.860303	450692.666431	44.760193
3503.730980	450700.248026	44.765197
3503.807279	450703.889681	44.770202
3503.830489	450702.871106	44.775207
3503.820746	450710.180066	44.780212
3504.000058	450698.936890	44.785217
3503.651227	450684.224980	44.790221
3503.835309	450666.384062	44.795226
3503.768845	450678.319881	44.800231
3503.499017	450683.843108	44.805236
3503.784809	450672.633834	44.810241
3503.610882	450676.568778	44.815245
3503.729692	450678.833576	44.820250
3503.686127	450686.959825	44.825255
3503.738563	450685.784391	44.830260
3503.777186	450676.542535	44.835265
3503.679885	450687.925019	44.840269
3504.036758	450676.806001	44.845274
3504.027294	450664.780715	44.850279
3503.784170	450660.099782	44.855284
3503.637598	450641.499177	44.860289
3503.693766	450647.275357	44.865293
3503.429144	450645.541088	44.870298
3503.882835	450648.463397	44.875303
3503.427832	450655.944251	44.880308
3503.617061	450649.215877	44.885313
3503.459240	450646.399059	44.890317
3503.566068	450652.319468	44.895322
3503.542146	450655.266529	44.900327
3503.486909	450660.908078	44.905332
3503.688741	450648.950874	44.910337
3503.718269	450661.683464	44.915341
3503.409794	450655.794957	44.920346
3503.780116	450652.031971	44.925351
3503.843747	450652.174162	44.930356
3504.190265	450658.005933	44.935361
3503.990693	450641.545038	44.940365
3503.724882	450633.416956	44.945370
3503.916856	450626.941871	44.950375
3503.602875	450624.352721	44.955380
3503.706836	450623.270631	44.960385
3503.621316	450631.302039	44.965389
3503.520233	450627.613567	44.970394
3503.815593	450632.793733	44.975399
3503.792271	450631.681018	44.980404
3504.002518	450625.253791	44.985409
3503.670780	450622.464463	44.990413
3503.930777	450594.868241	44.995418
3504.089021	450587.180570	45.000423
3504.161607	450595.186998	45.005428
3504.290224	450588.265203	45.010433
3504.298737	450579.890753	45.015437
3503.749670	450554.655209	45.020442
3503.731567	450551.308831	45.025447
3503.820712	450551.244005	45.030452
3503.667490	450550.913013	45.035457
3503.630262	450560.154722	45.040461
3503.522908	450559.664241	45.045466
3503.976073	450565.276193	45.050471
3503.517499	450566.820334	45.055476
3503.989697	450561.874067	45.060481
3504.003119	450545.430180	45.065485
3503.842649	450539.061531	45.070490
3503.985035	450518.842016	45.075495
3503.494747	450538.812072	45.080500
3503.767249	450525.676469	45.085505
3503.647167	450520.519342	45.090509
3503.711263	450540.756984	45.095514
3503.621197	450517.224961	45.100519
3503.417230	450541.463189	45.105524
3503.911327	450532.961216	45.110529
3503.841487	450532.363312	45.115533
3503.527719	450546.469636	45.120538
3503.711835	450540.553978	45.125543
3503.802863	450531.963482	45.130548
3503.867578	450511.553254	45.135553
3503.741984	450510.964163	45.140557
3503.794936	450497.660265	45.145562
3504.038401	450507.720311	45.150567
3503.591671	450514.641693	45.155572
3504.170252	450489.075584	45.160577
3503.967721	450507.985250	45.165581
3504.091960	450493.198438	45.170586
3504.137062	450474.770386	45.175591
3504.192945	450477.197390	45.180596
3504.207527	450465.929395	45.185601
3503.791216	450477.819128	45.190605
3503.930830	450451.713411	45.195610
3504.055853	450424.392055	45.200615
3503.728885	450443.372192	45.205620
3503.831584	450441.681336	45.210625
3503.914692	450432.483097	45.215629
3503.700559	450439.976691	45.220634
3503.889566	450438.627416	45.225639
3503.929369	450429.486768	45.230644
3503.717522	450411.454509	45.235649
3503.648685	450401.772812	45.240653
3503.959021	450399.389425	45.245658
3504.082781	450387.850401	45.250663
3503.894225	450391.889199	45.255668
3503.915585	450391.784341	45.260673
3504.044995	450398.157963	45.265677
3503.884444	450379.305625	45.270682
3503.957213	450371.276169	45.275687
3503.906238	450372.349917	45.280692
3503.825155	450369.876162	45.285697
3503.852978	450376.367342	45.290701
3504.300804	450373.048779	45.295706
3504.247502	450357.478000	45.300711
3503.793385	450347.857184	45.305716
3504.053948	450340.204005	45.310721
3504.095725	450324.922654	45.315725
3503.929936	450332.916107	45.320730
3503.666117	450334.378730	45.325735
3503.547778	450310.191258	45.330740
3503.998545	450291.698934	45.335745
3503.529891	450292.128257	45.340749
3503.613779	450295.616536	45.345754
3503.642206	450296.779230	45.350759
3503.669781	450303.016737	45.355764
3503.992338	450295.353742	45.360769
3503.882239	450294.609956	45.365773
3503.922907	450313.785817	45.370778
3503.780824	450312.336633	45.375783
3503.782197	450316.040940	45.380788
3504.192858	450288.978753	45.385793
3504.338739	450284.895960	45.390797
3503.856521	450273.097442	45.395802
3504.210261	450262.942913	45.400807
3503.888100	450266.444637	45.405812
3503.844427	450244.478155	45.410817
3503.745238	450241.702767	45.415821
3503.739837	450237.390145	45.420826
3503.907114	450230.512879	45.425831
3503.522484	450240.418594	45.430836
3503.759636	450235.458667	45.435841
3503.697251	450234.910324	45.440845
3503.569311	450242.288862	45.445850
3504.020819	450237.802520	45.450855
3503.596099	450242.893613	45.455860
3503.744835	450236.374509	45.460865
3503.902258	450250.102046	45.465869
3503.626201	450224.721492	45.470874
3504.067200	450214.096425	45.475879
3503.510266	450220.324857	45.480884
3503.721863	450209.330076	45.485889
3504.242311	450215.743428	45.490893
3503.776766	450212.721467	45.495898
3504.265520	450208.533713	45.500903
3503.973696	450192.543805	45.505908
3503.865942	450176.271054	45.510913
3503.999942	450175.691665	45.515917
3503.895622	450169.973750	45.520922
3503.896767	450168.349675	45.525927
3503.388746	450178.630151	45.530932
3503.669541	450164.275104	45.535937
3504.006091	450169.448863	45.540941
3503.788492	450162.023453	45.545946
3503.913928	450143.531692	45.550951
3503.835237	450138.063453	45.555956
3503.448833	450134.267764	45.560961
3503.629072	450148.093249	45.565965
3503.502327	450144.205768	45.570970
3503.849074	450146.536081	45.575975
3503.774707	450154.058420	45.580980
3504.135500	450156.538753	45.585985
3504.137747	450162.069842	45.590989
3503.621450	450153.372222	45.595994
3504.039956	450132.702746	45.600999
3503.870628	450143.538664	45.606004
3503.705628	450130.167515	45.611009
3503.573711	450121.510615	45.616013
3503.707167	450127.426948	45.621018
3503.794348	450135.380480	45.626023
3503.489103	450125.228567	45.631028
3503.791893	450108.434146	45.636033
3503.914517	450113.743229	45.641037
3503.486529	450112.440721	45.646042
3503.967211	450116.069292	45.651047
3503.916626	450087.557368	45.656052
3503.865373	450079.598164	45.661057
3503.775487	450072.812251	45.666061
3503.735796	450070.027436	45.671066
3503.688703	450062.067568	45.676071
3503.750751	450074.693844	45.681076
3503.813685	450070.218147	45.686081
3504.023266	450067.952149	45.691085
3503.771800	450068.347142	45.696090
3504.038569	450065.158652	45.701095
3503.793493	450049.567234	45.706100
3503.767352	450030.033650	45.711105
3503.881308	450042.803980	45.716109
3503.462886	450050.329993	45.721114
3503.671705	450039.132581	45.726119
3503.804076	450041.649035	45.731124
3503.974944	450040.048868	45.736129
3503.971156	450044.007771	45.741133
3503.681847	450031.772658	45.746138
3503.857491	450005.914482	45.751143
3503.780965	450004.099683	45.756148
3503.741179	450000.198432	45.761153
3503.399335	450002.637611	45.766157
3503.500526	450003.230595	45.771162
3503.686107	450005.180420	45.776167
3503.674262	450017.564671	45.781172
3503.690822	450022.839794	45.786177
3503.756685	450014.557569	45.791181
3503.540176	450021.239714	45.796186
3503.579486	450014.737845	45.801191
3503.757756	450013.897718	45.806196
3503.658870	450018.226890	45.811201
3503.818517	450017.237464	45.816205
3503.728718	450009.690308	45.821210
3503.834807	450021.142461	45.826215
3503.625355	449995.700381	45.831220
3503.649066	449974.382709	45.836225
3503.686183	449974.985823	45.841229
3503.870764	449989.165949	45.846234
3503.926709	449980.783785	45.851239
3503.629004	449986.311583	45.856244
3503.714916	449987.363711	45.861249
3503.854484	449992.213416	45.866253
3503.773752	449997.402428	45.871258
3503.940895	449978.751701	45.876263
3503.529728	450010.584608	45.881268
3503.905894	449994.184485	45.886273
3503.887920	449967.950895	45.891277
3503.611509	449955.713702	45.896282
3503.831766	449959.332718	45.901287
3503.516005	449960.702079	45.906292
3503.772129	449955.992831	45.911297
3503.722924	449967.621802	45.916301
3503.828060	449960.348300	45.921306
3503.919454	449955.614345	45.926311
3503.819734	449964.358693	45.931316
3503.614459	449959.062665	45.936321
3503.819106	449950.403246	45.941325
3503.623065	449933.636805	45.946330
3503.614396	449934.906877	45.951335
3503.189011	449920.206583	45.956340
3503.862303	449922.586795	45.961345
3503.552460	449941.463138	45.966349
3503.533675	449946.084147	45.971354
3503.786713	449930.921384	45.976359
3503.560585	449941.461888	45.981364
3503.590278	449934.403294	45.986369
3503.715864	449935.855133	45.991373
3503.771610	449930.923817	45.996378
3503.949314	449934.092835	46.001383
3504.044249	449938.492879	46.006388
3503.954196	449931.960689	46.011393
3503.914166	449926.537036	46.016397
3503.575312	449902.383999	46.021402
3503.943220	449894.713705	46.026407
3503.932997	449893.294398	46.031412
3503.517117	449905.793325	46.036417
3503.734920	449899.263208	46.041421
3503.681770	449887.244425	46.046426
3503.632596	449895.676323	46.051431
3503.634562	449908.565926	46.056436
3503.952861	449892.225626	46.061441
3503.699886	449899.319552	46.066445
3503.611427	449901.718686	46.071450
3503.891007	449899.289363	46.076455
3504.069130	449905.604673	46.081460
3504.088871	449886.520444	46.086465
3504.075015	449882.412084	46.091469
3504.024312	449874.249731	46.096474
3504.164915	449886.356215	46.101479
3503.875583	449859.657921	46.106484
3503.711059	449851.868787	46.111489
3503.955018	449830.922150	46.116493
3503.679454	449843.246687	46.121498
3503.784922	449851.857146	46.126503
3503.482901	449843.125537	46.131508
3503.622203	449843.966240	46.136513
3503.748196	449843.540353	46.141517
3504.068126	449851.203451	46.146522
3503.985883	449831.577073	46.151527
3503.681569	449825.687697	46.156532
3503.755172	449813.242857	46.161537
3504.009123	449798.587342	46.166541
3503.500512	449802.829078	46.171546
3504.078467	449807.203540	46.176551
3503.834060	449806.988447	46.181556
3503.782556	449803.190511	46.186561
3503.508699	449817.341714	46.191565
3503.680572	449809.803877	46.196570
3503.845751	449811.147969	46.201575
3503.652708	449821.987784	46.206580
3503.391773	449798.279052	46.211585
3503.573091	449804.796876	46.216589
3503.523579	449818.151396	46.221594
3504.042982	449791.477425	46.226599
3503.758944	449788.274472	46.231604
3503.505539	449782.783020	46.236609
3503.516989	449784.455902	46.241613
3503.577638	449777.138628	46.246618
3503.652686	449785.195693	46.251623
3503.546981	449776.534522	46.256628
3503.488609	449775.579550	46.261633
3503.996670	449778.696368	46.266637
3503.905938	449783.278034	46.271642
3503.985020	449785.853687	46.276647
3504.037052	449789.702314	46.281652
3503.875012	449776.888720	46.286657
3503.692601	449760.272244	46.291661
3503.715152	449757.731293	46.296666
3503.866600	449739.539588	46.301671
3503.894454	449750.395265	46.306676
3503.453771	449756.351703	46.311681
3503.929204	449753.434673	46.316685
3503.467161	449765.281249	46.321690
3504.058227	449750.420171	46.326695
3503.848517	449770.752514	46.331700
3503.574905	449746.081522	46.336705
3503.620345	449742.268251	46.341709
3503.360211	449750.124573	46.346714
3503.875937	449730.911066	46.351719
3503.597647	449730.346092	46.356724
3503.363634	449716.275142	46.361729
3503.425406	449734.991412	46.366733
3503.307676	449732.574129	46.371738
3503.557884	449749.433671	46.376743
3503.828770	449768.370598	46.381748
3503.768685	449735.343178	46.386753
3503.846040	449724.775373	46.391757
3503.544373	449726.852992	46.396762
3503.788653	449716.766277	46.401767
3503.819576	449729.905141	46.406772
3503.683985	449724.293556	46.411777
3503.731908	449731.847448	46.416781
3503.558581	449731.722614	46.421786
3503.694728	449731.041380	46.426791
3503.593263	449739.278608	46.431796
3503.451226	449742.802684	46.436801
3503.402880	449736.111602	46.441805
3503.378071	449736.623016	46.446810
3503.577956	449724.462653	46.451815
3503.514196	449754.363315	46.456820
3503.602156	449739.074279	46.461825
3503.944857	449717.908940	46.466829
3503.866591	449750.247807	46.471834
3503.938208	449750.896221	46.476839
3503.677368	449716.327321	46.481844
3503.779864	449707.379472	46.486849
3503.772115	449715.449650	46.491853
3503.864682	449708.939277	46.496858
3503.931179	449704.107711	46.501863
3504.014898	449712.264927	46.506868
3503.484431	449705.497804	46.511873
3503.874616	449707.567555	46.516877
3503.818493	449713.919946	46.521882
3503.682865	449705.212731	46.526887
3503.918413	449693.858684	46.531892
3503.679843	449686.690177	46.536897
3503.765390	449691.446988	46.541901
3503.595880	449677.974796	46.546906
3503.727111	449686.631992	46.551911
3504.181040	449668.392416	46.556916
3503.875014	449673.921603	46.561921
3503.946072	449684.871978	46.566925
3503.820183	449671.494383	46.571930
3503.811850	449643.888703	46.576935
3503.357051	449670.603401	46.581940
3503.790581	449630.951292	46.586945
3503.855363	449646.368521	46.591949
3503.724304	449667.297500	46.596954
3503.876582	449629.567529	46.601959
3503.715237	449661.716658	46.606964
3503.657582	449660.304835	46.611969
3503.828627	449655.913465	46.616973
3503.775530	449655.160648	46.621978
3503.951892	449652.798364	46.626983
3503.779609	449625.878306	46.631988
3503.658746	449624.425724	46.636993
3503.990157	449600.826148	46.641997
3503.401081	449632.433952	46.647002
3503.874174	449619.824362	46.652007
3503.772082	449606.950450	46.657012
3503.517092	449618.358384	46.662017
3503.787841	449622.375456	46.667021
3503.343663	449604.633039	46.672026
3503.680596	449629.395691	46.677031
3503.704732	449621.931894	46.682036
3503.711088	449623.757838	46.687041
3504.065800	449619.692666	46.692045
3503.477172	449643.688144	46.697050
3503.850667	449597.295955	46.702055
3503.765479	449621.211874	46.707060
3503.758691	449582.441258	46.712065
3503.820693	449578.117860	46.717069
3503.499386	449588.521323	46.722074
3504.025419	449580.166202	46.727079
3503.376271	449589.961761	46.732084
3503.606354	449595.710710	46.737089
3503.963748	449571.193527	46.742093
3503.365145	449604.629816	46.747098
3503.756692	449583.202892	46.752103
3503.314253	449607.581285	46.757108
3503.577660	449576.075699	46.762113
3503.721937	449597.113461	46.767117
3503.834798	449585.068280	46.772122
3503.469217	449592.586085	46.777127
3503.625343	449605.755976	46.782132
3503.364869	449591.435392	46.787137
3503.720537	449597.265985	46.792141
3503.428814	449621.468294	46.797146
3503.695661	449599.249124	46.802151
3503.977903	449589.004109	46.807156
3503.848952	449591.612669	46.812161
3503.936127	449576.881882	46.817165
3503.349036	449575.858236	46.822170
3503.666638	449530.946453	46.827175
3503.489383	449582.788597	46.832180
3503.729763	449577.980265	46.837185
3504.270729	449540.696192	46.842189
3503.706896	449588.894796	46.847194
3504.241392	449562.674913	46.852199
3503.474830	449564.420049	46.857204
3503.631674	449565.156493	46.862209
3503.566951	449586.430296	46.867213
3503.894210	449552.732407	46.872218
3503.906823	449538.774609	46.877223
3503.954617	449557.239489	46.882228
3503.778724	449530.116898	46.887233
3504.285672	449540.592449	46.892237
3503.869701	449543.144889	46.897242
3503.823848	449533.306952	46.902247
3503.928571	449505.226501	46.907252
3503.751835	449516.571365	46.912257
3503.817257	449486.264170	46.917261
3503.660824	449505.928591	46.922266
3504.204322	449495.692984	46.927271
3503.681807	449493.897898	46.932276
3503.541191	449519.852623	46.937281
3504.072618	449498.910995	46.942285
3503.498564	449496.413577	46.947290
3503.373753	449511.657872	46.952295
3503.649341	449504.560277	46.957300
3503.785136	449496.216065	46.962305
3503.784871	449481.600538	46.967309
3503.642932	449469.849318	46.972314
3504.012178	449452.587184	46.977319
3503.656530	449460.813942	46.982324
3503.480809	449480.075444	46.987329
3504.090358	449442.881871	46.992333
3503.776928	449487.996181	46.997338
3503.694465	449457.357086	47.002343
3503.433368	449492.516384	47.007348
3503.793303	449460.995385	47.012353
3503.675781	449488.519701	47.017357
3503.730971	449453.545215	47.022362
3503.791357	449481.295160	47.027367
3503.643662	449441.074876	47.032372
3503.716005	449467.097493	47.037377
3503.899756	449440.932919	47.042381
3503.947744	449428.847163	47.047386
3503.752782	449452.679110	47.052391
3504.126457	449423.033586	47.057396
3503.946409	449450.111094	47.062401
3504.045811	449428.831707	47.067405
3503.217753	449435.509194	47.072410
3503.690877	449403.310492	47.077415
3503.462290	449416.947293	47.082420
3503.480996	449414.559159	47.087425
3503.799982	449400.958838	47.092429
3503.746303	449419.998102	47.097434
3503.843654	449431.451927	47.102439
3503.939595	449405.960927	47.107444
3503.657651	449419.758407	47.112449
3503.763095	449418.320787	47.117453
3503.473624	449441.000465	47.122458
3503.841572	449415.618724	47.127463
3503.727512	449418.986180	47.132468
3503.266962	449432.355148	47.137473
3504.205652	449407.035422	47.142477
3503.873166	449412.315110	47.147482
3503.715511	449401.682811	47.152487
3503.867593	449386.941645	47.157492
3503.984347	449375.301730	47.162497
3503.690462	449387.020417	47.167501
3503.544811	449387.195699	47.172506
3503.767383	449378.482487	47.177511
3503.698001	449379.711437	47.182516
3503.414386	449399.193056	47.187521
3503.848847	449383.341526	47.192525
3503.857011	449386.841912	47.197530
3503.571595	449386.988539	47.202535
3503.243948	449397.545336	47.207540
3503.458647	449388.782623	47.212545
3503.732582	449391.124524	47.217549
3503.460027	449400.150148	47.222554
3503.730887	449389.500855	47.227559
3504.014409	449383.619940	47.232564
3503.608782	449376.173252	47.237569
3503.544170	449351.265809	47.242573
3503.469963	449364.218502	47.247578
3503.283510	449363.182263	47.252583
3503.516988	449368.829233	47.257588
3503.489611	449366.296132	47.262593
3503.925731	449356.128188	47.267597
3503.407352	449380.214328	47.272602
3503.836338	449352.488425	47.277607
3503.574131	449354.661337	47.282612
3503.641079	449369.317175	47.287617
3503.793242	449355.083463	47.292621
3503.417443	449370.519772	47.297626
3503.731216	449369.861197	47.302631
3503.607736	449369.220994	47.307636
3503.506055	449357.615600	47.312641
3503.749824	449377.927349	47.317645
3503.631498	449370.739736	47.322650
3503.478410	449362.644138	47.327655
3503.682852	449363.119320	47.332660
3503.696248	449388.948348	47.337665
3503.815098	449373.501943	47.342669
3503.609860	449371.301451	47.347674
3503.832757	449372.179706	47.352679
3503.586157	449391.046496	47.357684
3503.815273	449377.460368	47.362689
3503.967393	449341.861406	47.367693
3503.514361	449340.055324	47.372698
3503.475772	449344.425838	47.377703
3503.683012	449320.490365	47.382708
3503.441959	449342.299754	47.387713
3503.701877	449329.317715	47.392717
3503.777676	449336.867328	47.397722
3503.474062	449331.180710	47.402727
3503.613832	449331.310874	47.407732
3503.442532	449348.288086	47.412737
3504.016274	449325.005166	47.417741
3503.387740	449344.541355	47.422746
3503.340369	449339.524718	47.427751
3503.616551	449341.612523	47.432756
3503.181674	449340.666302	47.437761
3503.603053	449352.830176	47.442765
3503.318585	449341.456664	47.447770
3503.479899	449343.613377	47.452775
3503.685654	449360.378729	47.457780
3503.701718	449341.193139	47.462785
3503.573096	449344.562907	47.467789
3503.497205	449358.175605	47.472794
3503.547921	449342.587705	47.477799
3503.427856	449365.139179	47.482804
3503.381707	449342.512505	47.487809
3503.801305	449375.026934	47.492813
3503.688829	449353.933219	47.497818
3503.935412	449369.981627	47.502823
3503.605856	449367.039554	47.507828
3503.348865	449363.832266	47.512833
3504.010359	449373.369983	47.517837
3503.610344	449361.202766	47.522842
3503.657851	449376.318411	47.527847
3503.569475	449362.833211	47.532852
3503.263259	449382.521413	47.537857
3503.708485	449367.378653	47.542861
3503.343135	449363.833253	47.547866
3503.675300	449374.387257	47.552871
3503.897709	449376.635806	47.557876
3503.615312	449375.360989	47.562881
3503.933681	449374.041954	47.567885
3503.681142	449356.522797	47.572890
3503.640642	449344.247991	47.577895
3503.753164	449329.563790	47.582900
3503.369220	449358.602093	47.587905
3503.854665	449325.386359	47.592909
3503.380387	449353.880710	47.597914
3503.921178	449342.072250	47.602919
3503.867224	449331.271280	47.607924
3503.635584	449350.795473	47.612929
3503.944642	449347.194210	47.617933
3504.310507	449342.619738	47.622938
3503.951643	449319.788730	47.627943
3504.080279	449324.183562	47.632948
3503.975953	449300.195823	47.637953
3504.025564	449305.821125	47.642957
3503.944481	449327.300746	47.647962
3504.012919	449280.448663	47.652967
3504.143811	449286.467113	47.657972
3503.917012	449278.484636	47.662977
3504.187072	449260.223058	47.667981
3503.651355	449287.255480	47.672986
3504.072121	449259.378519	47.677991
3503.905746	449264.479734	47.682996
3504.000344	449237.872285	47.688001
3503.601020	449231.591783	47.693005
3503.730378	449246.237832	47.698010
3503.689720	449212.140871	47.703015
3503.819264	449237.850206	47.708020
3503.676117	449244.317979	47.713025
3503.957150	449220.776733	47.718029
3503.815013	449236.429938	47.723034
3503.876951	449223.377639	47.728039
3504.131188	449200.094352	47.733044
3503.720895	449202.239938	47.738049
3503.839575	449191.462363	47.743053
3503.872699	449203.789188	47.748058
3504.045809	449198.788417	47.753063
3503.627621	449198.397792	47.758068
3503.787827	449211.059769	47.763073
3503.887765	449188.968093	47.768077
3503.851959	449180.295650	47.773082
3503.960831	449159.166769	47.778087
3504.195223	449165.321138	47.783092
3503.713955	449165.955469	47.788097
3503.860589	449164.511322	47.793101
3503.808689	449172.030425	47.798106
3503.947331	449159.371958	47.803111
3504.063489	449130.984755	47.808116
3503.551645	449128.781958	47.813121
3503.688677	449134.951724	47.818125
3503.555630	449129.897836	47.823130
3503.626017	449122.325071	47.828135
3503.771565	449121.896080	47.833140
3503.657290	449124.959116	47.838145
3503.513757	449128.229774	47.843149
3503.316815	449132.371612	47.848154
3503.568561	449127.358395	47.853159
3503.651061	449120.341957	47.858164
3503.518390	449132.999524	47.863169
3503.892146	449123.399579	47.868173
3504.066861	449124.792954	47.873178
3503.812430	449137.875760	47.878183
3503.908925	449127.304660	47.883188
3503.871046	449100.971743	47.888193
3503.698350	449093.589643	47.893197
3503.589589	449087.669166	47.898202
3503.673229	449098.465579	47.903207
3503.806230	449093.724872	47.908212
3503.441918	449100.582892	47.913217
3503.713253	449095.515822	47.918221
3503.659630	449093.037589	47.923226
3503.671069	449097.247993	47.928231
3503.870887	449109.142522	47.933236
3503.800638	449102.860716	47.938241
3503.885382	449092.443706	47.943245
3503.893199	449091.427493	47.948250
3503.627107	449063.557378	47.953255
3504.018594	449060.501286	47.958260
3503.871007	449057.936404	47.963265
3503.892337	449061.028762	47.968269
3503.490491	449061.092296	47.973274
3503.871935	449055.601816	47.978279
3503.755584	449061.811656	47.983284
3503.591584	449072.139732	47.988289
3503.864901	449062.809388	47.993293
3503.725783	449053.087491	47.998298
3503.406027	449039.080436	48.003303
3503.530714	449028.657083	48.008308
3503.120066	449036.385189	48.013313
3503.230970	449058.189955	48.018317
3503.658805	449070.657453	48.023322
3503.753975	449070.287174	48.028327
3503.536963	449070.169242	48.033332
3503.525982	449074.941438	48.038337
3503.769125	449069.726570	48.043341
3503.508607	449069.970761	48.048346
3503.598314	449062.750169	48.053351
3503.704308	449049.132564	48.058356
3503.581781	449035.703323	48.063361
3503.557290	449039.513420	48.068365
3503.360775	449041.117732	48.073370
3503.636762	449025.849256	48.078375
3503.516213	449052.917817	48.083380
3503.531591	449038.553288	48.088385
3503.485408	449039.930837	48.093389
3503.479857	449039.627229	48.098394
3503.262692	449052.348946	48.103399
3503.489646	449069.770899	48.108404
3503.650211	449079.996917	48.113409
3503.807726	449075.303080	48.118413
3503.630673	449066.957421	48.123418
3503.827428	449051.346241	48.128423
3503.850383	449043.780948	48.133428
3503.874421	449051.592582	48.138433
3503.875445	449043.218764	48.143437
3503.500994	449050.941143	48.148442
3503.619028	449063.203870	48.153447
3503.664949	449051.727240	48.158452
3503.419250	449046.538893	48.163457
3503.926050	449052.193484	48.168461
3503.608111	449061.277163	48.173466
3503.466776	449068.150694	48.178471
3503.783216	449058.407535	48.183476
3503.300532	449051.734166	48.188481
3503.799585	449067.235378	48.193485
3503.903988	449059.809463	48.198490
3503.567003	449030.935526	48.203495
3503.933526	449027.883376	48.208500
3503.821685	449010.240219	48.213505
3503.782806	449032.068687	48.218509
3503.567495	449023.069315	48.223514
3503.709365	449010.562506	48.228519
3503.635458	449015.496910	48.233524
3503.490613	449033.992655	48.238529
3503.808883	449004.456859	48.243533
3503.866175	449031.852579	48.248538
3503.435476	449022.684257	48.253543
3503.583790	449005.456718	48.258548
3503.727655	449037.203211	48.263553
3504.121252	448987.457167	48.268557
3503.538677	449016.781040	48.273562
3503.943197	448977.589156	48.278567
3503.804358	449008.416134	48.283572
3503.760054	448978.582374	48.288577
3504.117738	448999.637689	48.293581
3504.308058	448978.648019	48.298586
3503.838972	448999.275782	48.303591
3504.111423	448970.457681	48.308596
3503.920620	448962.773903	48.313601
3503.979905	448959.415063	48.318605
3503.732913	448968.792060	48.323610
3503.836074	448948.120639	48.328615
3504.110677	448973.401337	48.333620
3503.988512	448929.166913	48.338625
3503.946327	448921.967126	48.343629
3504.057634	448931.185999	48.348634
3503.703595	448924.999756	48.353639
3503.710570	448910.128978	48.358644
3503.363105	448943.780260	48.363649
3503.554568	448919.796122	48.368653
3503.679497	448922.872121	48.373658
3503.785470	448926.306365	48.378663
3504.398571	448915.247508	48.383668
3503.671110	448907.547046	48.388673
3503.374913	448871.713740	48.393677
3503.392535	448897.441142	48.398682
3503.702100	448872.271041	48.403687
3503.630026	448884.513164	48.408692
3503.465751	448888.954380	48.413697
3503.600196	448873.200682	48.418701
3503.787111	448905.904795	48.423706
3503.646197	448891.970881	48.428711
3503.970968	448879.688839	48.433716
3503.581695	448901.674317	48.438721
3503.603044	448892.129986	48.443725
3503.242982	448893.810911	48.448730
3503.825853	448880.016324	48.453735
3503.593759	448896.445225	48.458740
3503.670053	448884.963712	48.463745
3503.796922	448881.949427	48.468749
3503.731080	448892.312815	48.473754
3503.677873	448913.788409	48.478759
3504.084872	448870.840471	48.483764
3503.654095	448888.265032	48.488769
3503.671552	448854.361362	48.493773
3504.037677	448843.087763	48.498778
3503.476191	448875.757974	48.503783
3503.649745	448840.459362	48.508788
3503.739775	448859.222616	48.513793
3503.566402	448870.516511	48.518797
3503.742499	448847.752726	48.523802
3503.717139	448872.421201	48.528807
3503.935744	448833.156966	48.533812
3503.526813	448871.690062	48.538817
3503.486717	448866.367674	48.543821
3504.107624	448839.067575	48.548826
3503.839841	448861.033887	48.553831
3503.686663	448819.037153	48.558836
3503.851310	448831.901633	48.563841
3503.929708	448822.906505	48.568845
3503.386847	448839.333821	48.573850
3503.397623	448807.359638	48.578855
3503.773377	448833.182748	48.583860
3503.741584	448812.126540	48.588865
3503.488310	448839.216329	48.593869
3503.623317	448816.306759	48.598874
3503.463383	448825.517801	48.603879
3503.731153	448825.221734	48.608884
3503.523571	448826.574059	48.613889
3503.657492	448816.656653	48.618893
3503.613032	448828.031690	48.623898
3503.532879	448822.258874	48.628903
3503.891671	448856.762886	48.633908
3503.530383	448836.976784	48.638913
3503.537694	448853.114120	48.643917
3503.536636	448837.178818	48.648922
3503.702246	448846.693640	48.653927
3503.681405	448837.409706	48.658932
3503.696069	448838.625399	48.663937
3503.900904	448836.613782	48.668941
3504.047370	448803.907645	48.673946
3503.320550	448822.343303	48.678951
3504.187720	448782.468960	48.683956
3503.446313	448814.812447	48.688961
3503.596450	448795.452965	48.693965
3503.865421	448794.598457	48.698970
3504.015117	448801.121561	48.703975
3503.750256	448812.988196	48.708980
3503.643170	448792.552873	48.713985
3503.878265	448809.618483	48.718989
3503.337196	448776.056740	48.723994
3503.717090	448759.046163	48.728999
3503.826868	448787.601125	48.734004
3503.756722	448764.774685	48.739009
3503.800354	448783.240833	48.744013
3503.763763	448755.587822	48.749018
3503.567703	448775.411370	48.754023
3503.956045	448756.318702	48.759028
3503.496903	448775.118085	48.764033
3503.727016	448789.646992	48.769037
3503.525167	448769.074378	48.774042
3503.671782	448756.312933	48.779047
3503.524590	448782.777017	48.784052
3503.695862	448759.760159	48.789057
3503.692314	448774.072262	48.794061
3503.668215	448767.833821	48.799066
3503.384327	448777.013726	48.804071
3503.842485	448769.379549	48.809076
3503.310866	448792.098133	48.814081
3503.831684	448748.776728	48.819085
3503.498285	448777.503259	48.824090
3503.115529	448761.881994	48.829095
3503.483470	448761.722342	48.834100
3503.517706	448798.206250	48.839105
3503.631669	448769.362205	48.844109
3503.527331	448776.280723	48.849114
3503.467556	448812.119719	48.854119
3503.496002	448781.106956	48.859124
3503.508561	448760.297441	48.864129
3503.598138	448787.942094	48.869133
3503.453678	448790.096444	48.874138
3503.781186	448776.189913	48.879143
3503.921538	448768.504474	48.884148
3503.509234	448778.110679	48.889153
3503.345289	448739.820261	48.894157
3503.600365	448766.322274	48.899162
3503.464334	448762.639030	48.904167
3504.141527	448726.956133	48.909172
3503.878289	448780.488401	48.914177
3503.683468	448754.941156	48.919181
3503.988828	448744.336866	48.924186
3503.656147	448748.652480	48.929191
3503.791222	448757.157163	48.934196
3503.953355	448746.727766	48.939201
3503.743322	448741.076961	48.944205
3503.855062	448754.051347	48.949210
3503.755665	448737.725522	48.954215
3504.153356	448719.595599	48.959220
3503.682852	448713.376959	48.964225
3503.729963	448727.833334	48.969229
3504.084285	448705.447239	48.974234
3503.830142	448737.003304	48.979239
3504.010050	448694.598442	48.984244
3503.811614	448713.610414	48.989249
3504.150022	448664.278411	48.994253
3503.819034	448701.327707	48.999258
3503.887046	448657.011956	49.004263
3503.979304	448688.158076	49.009268
3503.959386	448669.282125	49.014273
3503.780117	448677.532025	49.019277
3503.833227	448630.579564	49.024282
3503.705850	448654.756891	49.029287
3503.745399	448627.091693	49.034292
3503.555176	448651.938712	49.039297
3503.781519	448612.926637	49.044301
3503.705456	448647.601199	49.049306
3503.680920	448646.437830	49.054311
3504.046300	448629.987708	49.059316
3503.924332	448630.210002	49.064321
3503.741172	448645.616335	49.069325
3503.586197	448623.361421	49.074330
3503.274367	448620.670203	49.079335
3503.574186	448644.932261	49.084340
3503.687739	448634.358242	49.089345
3503.824123	448624.491116	49.094349
3504.027415	448609.690615	49.099354
3503.739037	448606.132931	49.104359
3503.522081	448608.451009	49.109364
3503.430292	448603.288983	49.114369
3503.846365	448586.932319	49.119373
3503.868476	448617.835868	49.124378
3503.736735	448591.263464	49.129383
3503.708268	448579.037104	49.134388
3503.600925	448619.502210	49.139393
3503.573149	448601.185701	49.144397
3503.723464	448591.011855	49.149402
3503.308510	448637.412613	49.154407
3503.548158	448584.543527	49.159412
3503.601580	448614.021118	49.164417
3503.888898	448607.428903	49.169421
3503.998843	448604.214256	49.174426
3503.699212	448589.340992	49.179431
3504.019994	448579.952203	49.184436
3503.880571	448567.540375	49.189441
3504.234932	448575.350702	49.194445
3503.654222	448572.854234	49.199450
3504.042467	448545.083068	49.204455
3504.078734	448565.885078	49.209460
3503.922987	448525.258489	49.214465
3503.595401	448548.960067	49.219469
3503.943834	448517.845624	49.224474
3503.801347	448545.374994	49.229479
3504.344792	448523.872341	49.234484
3503.646160	448519.770488	49.239489
3503.830427	448524.968686	49.244493
3504.165300	448489.187290	49.249498
3503.494468	448507.259089	49.254503
3504.013117	448493.068423	49.259508
3503.824148	448492.692301	49.264513
3503.891038	448509.327963	49.269517
3504.083909	448471.234456	49.274522
3503.886043	448508.922770	49.279527
3503.606214	448467.199181	49.284532
3504.051097	448438.708425	49.289537
3503.822361	448463.916987	49.294541
3503.594679	448432.690498	49.299546
3503.340786	448464.500644	49.304551
3503.632518	448456.892674	49.309556
3503.806978	448427.784893	49.314561
3503.667476	448465.920808	49.319565
3503.600633	448456.999251	49.324570
3503.680958	448448.866439	49.329575
3503.502563	448470.920486	49.334580
3503.605177	448453.598265	49.339585
3503.755039	448440.328627	49.344589
3503.813710	448483.914274	49.349594
3503.445634	448459.916616	49.354599
3504.013305	448471.042810	49.359604
3503.965636	448438.113098	49.364609
3503.584125	448407.367650	49.369613
3503.762665	448428.807053	49.374618
3504.046013	448424.448452	49.379623
3504.000027	448414.813070	49.384628
3503.511882	448452.344358	49.389633
3503.811575	448408.093016	49.394637
3503.907067	448445.684308	49.399642
3503.614694	448395.233433	49.404647
3503.634814	448416.545638	49.409652
3503.700043	448392.834672	49.414657
3503.662623	448392.282338	49.419661
3503.238424	448397.221494	49.424666
3503.376896	448389.231722	49.429671
3503.627904	448377.773094	49.434676
3503.499796	448409.360426	49.439681
3503.985151	448381.319962	49.444685
3503.495182	448401.444040	49.449690
3503.573165	448400.010699	49.454695
3503.828256	448410.729575	49.459700
3503.673079	448381.217086	49.464705
3503.819065	448395.252028	49.469709
3503.647786	448407.154825	49.474714
3503.675992	448377.765596	49.479719
3503.762314	448399.625611	49.484724
3503.699140	448400.904382	49.489729
3503.483426	448408.906383	49.494733
3503.996790	448404.612920	49.499738
3503.828759	448404.030482	49.504743
3503.837689	448371.700741	49.509748
3503.703646	448370.047160	49.514753
3504.023550	448367.662057	49.519757
3503.519394	448350.029669	49.524762
3503.715261	448371.060378	49.529767
3503.531256	448361.903550	49.534772
3503.918554	448345.652769	49.539777
3503.923117	448334.436081	49.544781
3503.698412	448374.970911	49.549786
3503.763745	448342.276957	49.554791
3503.888337	448350.275934	49.559796
3504.018024	448365.683747	49.564801
3503.680836	448333.966927	49.569805
3504.085073	448294.570946	49.574810
3503.838737	448333.840488	49.579815
3503.748078	448305.535730	49.584820
3503.707824	448309.906700	49.589825
3503.483440	448349.325000	49.594829
3503.649736	448330.064082	49.599834
3503.785627	448310.858706	49.604839
3503.511994	448339.170316	49.609844
3503.597266	448314.085824	49.614849
3503.563912	448300.439061	49.619853
3503.546199	448310.998103	49.624858
3503.531867	448344.800585	49.629863
3503.666436	448350.920197	49.634868
3503.550072	448364.083110	49.639873
3503.728275	448327.412716	49.644877
3503.937604	448285.814483	49.649882
3503.746570	448286.047698	49.654887
3503.965216	448316.057807	49.659892
3503.898916	448281.100776	49.664897
3503.425413	448323.552817	49.669901
3503.551986	448295.771970	49.674906
3503.732707	448266.003235	49.679911
3503.759392	448301.321831	49.684916
3503.640707	448296.569998	49.689921
3503.880675	448290.492692	49.694925
3503.834005	448312.779820	49.699930
3503.325059	448270.889095	49.704935
3503.589673	448269.070986	49.709940
3503.605605	448320.682377	49.714945
3503.375558	448274.129222	49.719949
3503.645981	448276.116533	49.724954
3503.493785	448317.096761	49.729959
3503.593431	448285.361574	49.734964
3503.964485	448253.380435	49.739969
3503.556863	448285.519631	49.744973
3503.730040	448248.900660	49.749978
3503.454508	448277.567902	49.754983
3503.988857	448230.132559	49.759988
3503.708904	448273.061608	49.764993
3503.784302	448245.288791	49.769997
3503.602463	448290.841362	49.775002
3503.537023	448269.079470	49.780007
3503.989447	448239.876765	49.785012
3503.795796	448284.416191	49.790017
3503.669160	448255.152788	49.795021
3503.846311	448270.502409	49.800026
3503.773177	448245.899645	49.805031
3503.739281	448214.794488	49.810036
3503.515332	448253.553112	49.815041
3503.415456	448216.520493	49.820045
3503.792695	448213.618799	49.825050
3503.109613	448252.145496	49.830055
3503.559427	448218.071059	49.835060
3503.470201	448236.761645	49.840065
3503.587961	448238.722340	49.845069
3503.676327	448213.992511	49.850074
3503.540628	448250.148874	49.855079
3503.682515	448209.880700	49.860084
3503.421701	448245.244827	49.865089
3503.641893	448208.618362	49.870093
3503.656510	448248.354309	49.875098
3503.496149	448228.586682	49.880103
3503.264536	448241.767882	49.885108
3504.038374	448217.234206	49.890113
3503.404515	448268.796175	49.895117
3503.997217	448224.345916	49.900122
3503.574184	448260.293928	49.905127
3503.856855	448219.140744	49.910132
3503.369995	448259.767965	49.915137
3503.613101	448219.940569	49.920141
3503.534054	448263.548394	49.925146
3502.986121	448240.390962	49.930151
3503.647696	448217.651326	49.935156
3503.513868	448271.773312	49.940161
3503.401623	448251.592089	49.945165
3503.057202	448238.400473	49.950170
3503.868553	448221.321304	49.955175
3503.481198	448234.730133	49.960180
3503.245286	448256.945727	49.965185
3503.447183	448225.346548	49.970189
3503.668355	448232.619781	49.975194
3503.061006	448273.012269	49.980199
3503.397334	448219.264309	49.985204
3502.993425	448270.992928	49.990209
3503.212376	448279.738281	49.995213
3503.560775	448280.190730	50.000218
3503.303012	448294.543311	50.005223
3503.581786	448281.354708	50.010228
3503.110654	448306.348001	50.015233
3503.568564	448274.505414	50.020237
3503.887383	448300.236609	50.025242
3503.600633	448293.582801	50.030247
3503.741092	448292.038075	50.035252
3503.796104	448283.807705	50.040257
3503.388246	448308.740242	50.045261
3503.473672	448282.792924	50.050266
3503.829980	448317.907135	50.055271
3504.060355	448289.805366	50.060276
3503.578916	448291.962279	50.065281
3503.571516	448268.617926	50.070285
3503.732928	448294.577015	50.075290
3503.272364	448280.236506	50.080295
3503.612122	448245.875000	50.085300
3503.865505	448271.159810	50.090305
3503.576291	448276.432910	50.095309
3503.656748	448272.512363	50.100314
3503.425835	448269.503806	50.105319
3504.229031	448249.025617	50.110324
3503.831847	448284.258989	50.115329
3503.856096	448250.150368	50.120333
3504.146135	448265.279143	50.125338
3503.702911	448258.700811	50.130343
3504.000850	448231.603316	50.135348
3503.966145	448234.501635	50.140353
3503.922578	448215.527555	50.145357
3503.916730	448238.366565	50.150362
3504.198489	448235.784474	50.155367
3503.832707	448216.506071	50.160372
3503.577183	448204.772171	50.165377
3503.616427	448217.910568	50.170381
3503.846419	448201.735306	50.175386
3504.057976	448192.059120	50.180391
3503.717365	448222.259258	50.185396
3503.837076	448184.075348	50.190401
3503.723522	448201.805531	50.195405
3503.956526	448228.971407	50.200410
3503.952065	448230.799169	50.205415
3503.619092	448186.393664	50.210420
3503.660996	448164.614707	50.215425
3503.474418	448146.119940	50.220429
3503.646430	448168.626393	50.225434
3503.461580	448178.399893	50.230439
3503.567760	448163.868220	50.235444
3503.316218	448159.340368	50.240449
3503.657117	448150.354239	50.245453
3503.929386	448121.179866	50.250458
3503.503627	448168.192274	50.255463
3503.784681	448159.114106	50.260468
3503.561778	448190.615214	50.265473
3503.680149	448185.978140	50.270477
3503.775679	448183.171725	50.275482
3503.566133	448161.026502	50.280487
3503.437148	448163.685977	50.285492
3503.412106	448160.137348	50.290497
3503.782745	448135.718076	50.295501
3503.878022	448153.466035	50.300506
3503.389377	448206.882987	50.305511
3503.387865	448192.266853	50.310516
3503.602270	448185.838301	50.315521
3503.286611	448171.931582	50.320525
3504.004260	448191.560433	50.325530
3503.538887	448200.261738	50.330535
3503.561085	448206.449902	50.335540
3503.604204	448196.698842	50.340545
3503.614592	448197.458482	50.345549
3503.692081	448198.664276	50.350554
3503.491607	448187.987444	50.355559
3503.870625	448142.048267	50.360564
3504.091994	448145.870395	50.365569
3503.825213	448155.606104	50.370573
3504.030202	448172.270926	50.375578
3503.148961	448142.923664	50.380583
3503.789154	448131.149637	50.385588
3503.617620	448136.505670	50.390593
3503.641754	448145.434123	50.395597
3503.401041	448114.412277	50.400602
3503.484391	448162.206995	50.405607
3503.567863	448129.763635	50.410612
3503.561634	448148.136661	50.415617
3503.515312	448131.446764	50.420621
3503.991225	448128.427958	50.425626
3503.294846	448170.712500	50.430631
3503.310641	448175.886657	50.435636
3503.081211	448152.983299	50.440641
3503.160790	448132.111881	50.445645
3503.771645	448127.599951	50.450650
3503.253366	448179.905116	50.455655
3503.318313	448175.530242	50.460660
3503.472076	448176.520975	50.465665
3503.602415	448187.158171	50.470669
3503.582506	448177.721574	50.475674
3503.144384	448157.744039	50.480679
3503.547022	448149.763179	50.485684
3503.435516	448167.543815	50.490689
3503.404876	448220.380822	50.495693
3503.758264	448198.146647	50.500698
3503.791546	448164.848496	50.505703
3503.653615	448165.936091	50.510708
3503.491333	448175.553770	50.515713
3503.513940	448143.932073	50.520717
3503.692168	448168.366099	50.525722
3503.552482	448147.529356	50.530727
3503.696388	448169.126726	50.535732
3503.425297	448119.839178	50.540737
3503.200822	448105.816503	50.545741
3503.480661	448084.710380	50.550746
3503.160128	447999.396745	50.555751
3502.991195	447944.712994	50.560756
3502.999265	447923.142169	50.565761
3502.637720	447839.458499	50.570765
3503.250018	447709.841978	50.575770
3503.167338	447668.187311	50.580775
3502.353831	447538.744486	50.585780
3502.516265	447425.742913	50.590785
3502.214208	447305.505757	50.595789
3502.344279	447175.353496	50.600794
3501.714443	447046.234213	50.605799
3501.784979	446890.306845	50.610804
3501.186207	446744.381378	50.615809
3501.045973	446568.690967	50.620813
3500.502333	446428.743913	50.625818
3500.662083	446239.756556	50.630823
3499.606953	446065.475941	50.635828
3499.582200	445856.009308	50.640833
3499.024553	445709.563427	50.645837
3498.959602	445494.821285	50.650842
3498.428300	445314.767580	50.655847
3497.965571	445110.236365	50.660852
3498.318631	444869.129906	50.665857
3497.431442	444684.356427	50.670861
3497.185839	444477.349069	50.675866
3496.584639	444217.910543	50.680871
3496.046548	444011.605294	50.685876
3495.601564	443765.081061	50.690881
3494.983610	443527.261835	50.695885
3495.224683	443296.360359	50.700890
3494.365357	443042.939904	50.705895
3493.539500	442809.410527	50.710900
3493.668388	442528.518093	50.715905
3492.645965	442320.549052	50.720909
3492.261869	442024.655050	50.725914
3491.671031	441788.642038	50.730919
3491.477157	441498.244962	50.735924
3490.821105	441234.366635	50.740929
3490.274260	440999.151316	50.745933
3489.972157	440681.144666	50.750938
3489.668639	440430.832966	50.755943
3488.725387	440139.522945	50.760948
3488.866125	439819.252137	50.765953
3487.780957	439580.376863	50.770957
3487.171566	439262.857455	50.775962
3486.377951	439001.997823	50.780967
3485.769668	438692.898882	50.785972
3485.737756	438385.278918	50.790977
3484.538276	438129.323026	50.795981
3484.410891	437786.119293	50.800986
3483.355173	437531.683140	50.805991
3483.039740	437205.561124	50.810996
3482.451573	436933.451702	50.816001
3481.848154	436622.066964	50.821005
3481.049490	436312.207146	50.826010
3479.824612	436015.409744	50.831015
3480.179735	435677.229458	50.836020
3479.473445	435415.861792	50.841025
3478.538409	435101.540288	50.846029
3478.689250	434759.038535	50.851034
3477.134235	434480.403574	50.856039
3476.717717	434135.444176	50.861044
3476.568763	433854.574294	50.866049
3475.574791	433514.902897	50.871053
3474.815187	433222.823736	50.876058
3473.917258	432893.310795	50.881063
3473.350675	432604.342661	50.886068
3473.147369	432271.614199	50.891073
3472.119290	431959.097220	50.896077
3471.734137	431641.015422	50.901082
3470.767273	431307.608170	50.906087
3470.115077	431021.099099	50.911092
3469.548103	430670.378469	50.916097
3468.848172	430386.891847	50.921101
3468.203817	430059.537645	50.926106
3467.745322	429736.035350	50.931111
3466.667240	429413.668231	50.936116
3466.161289	429107.891321	50.941121
3465.521247	428779.073048	50.946125
3464.924779	428457.964118	50.951130
3463.842605	428153.816460	50.956135
3463.046232	427845.759908	50.961140
3462.732483	427526.677564	50.966145
3461.875155	427211.436101	50.971149
3461.644855	426897.615635	50.976154
3460.441214	426580.973883	50.981159
3459.979115	426247.245432	50.986164
3459.455224	425968.712721	50.991169
3458.824862	425625.301126	50.996173
3458.321743	425314.045234	51.001178
3457.360060	424990.006387	51.006183
3456.502286	424690.635365	51.011188
3456.022994	424340.148065	51.016193
3455.108725	424053.935991	51.021197
3454.521333	423722.964976	51.026202
3453.896839	423384.578899	51.031207
3453.336479	423101.501411	51.036212
3452.792011	422760.326337	51.041217
3451.755862	422478.003512	51.046221
3451.425780	422137.752122	51.051226
3450.238250	421840.358166	51.056231
3449.622167	421508.806346	51.061236
3448.789308	421205.811860	51.066241
3448.106585	420899.640412	51.071245
3447.824083	420576.788750	51.076250
3446.695691	420273.018003	51.081255
3446.208403	419942.926087	51.086260
3445.347760	419654.983604	51.091265
3444.588007	419333.260110	51.096269
3444.135140	419018.445263	51.101274
3443.261919	418729.428371	51.106279
3442.676871	418421.487082	51.111284
3441.647010	418107.744178	51.116289
3440.904028	417811.685536	51.121293
3440.795794	417486.281393	51.126298
3439.655167	417209.359163	51.131303
3439.028403	416870.793472	51.136308
3438.387863	416589.644975	51.141313
3437.896340	416291.244328	51.146317
3437.323781	415971.994154	51.151322
3436.235060	415668.142754	51.156327
3435.580804	415372.527795	51.161332
3435.276303	415068.596959	51.166337
3433.896993	414782.364553	51.171341
3433.616039	414466.075349	51.176346
3432.664538	414176.745776	51.181351
3432.486129	413870.140067	51.186356
3431.539579	413584.666054	51.191361
3430.477307	413272.959585	51.196365
3429.896185	412962.977848	51.201370
3429.348789	412678.753290	51.206375
3428.680871	412385.016227	51.211380
3427.528347	412087.897062	51.216385
3427.216562	411773.006937	51.221389
3426.667918	411505.186743	51.226394
3425.741587	411194.199349	51.231399
3424.822738	410936.139712	51.236404
3424.662704	410596.691167	51.241409
3423.337938	410338.258591	51.246413
3423.239324	410029.847393	51.251418
3422.589753	409749.321434	51.256423
3421.825595	409461.009300	51.261428
3421.177723	409147.059777	51.266433
3420.365032	408888.838855	51.271437
3419.998734	408565.258055	51.276442
3418.932378	408271.264444	51.281447
3418.187706	407990.635716	51.286452
3417.652155	407691.723986	51.291457
3416.813153	407402.235264	51.296461
3416.432693	407120.295725	51.301466
3415.513384	406818.971016	51.306471
3414.753844	406553.351796	51.311476
3414.442492	406237.260795	51.316481
3413.166842	405977.665472	51.321485
3412.982259	405645.867022	51.326490
3411.990592	405406.986808	51.331495
3411.505057	405075.179078	51.336500
3410.907113	404812.289912	51.341505
3409.736584	404511.262291	51.346509
3409.328278	404245.110488	51.351514
3408.519130	403950.806730	51.356519
3407.938682	403663.326794	51.361524
3407.503570	403371.042759	51.366529
3406.452795	403102.136198	51.371533
3405.855083	402818.159047	51.376538
3405.389653	402537.818705	51.381543
3404.680788	402240.255199	51.386548
3404.034830	401951.931443	51.391553
3403.244862	401685.945786	51.396557
3402.555972	401377.034279	51.401562
3401.797100	401121.893092	51.406567
3401.250811	400815.470217	51.411572
3400.502843	400565.864439	51.416577
3399.425621	400265.341501	51.421581
3399.162079	399966.339462	51.426586
3398.612975	399717.738001	51.431591
3397.739274	399432.580097	51.436596
3396.346366	399160.136054	51.441601
3396.093195	398859.292005	51.446605
3395.595303	398611.843484	51.451610
3395.023571	398309.392424	51.456615
3394.009358	398069.037872	51.461620
3393.079449	397771.494126	51.466625
3392.829210	397481.339822	51.471629
3392.176089	397213.440532	51.476634
3391.694983	396974.595424	51.481639
3390.715898	396681.066547	51.486644
3390.145195	396369.547250	51.491649
3389.216991	396135.597283	51.496653
3388.680661	395838.762315	51.501658
3388.090042	395578.848562	51.506663
3387.728721	395272.523355	51.511668
3387.018123	395039.497537	51.516673
3386.186602	394742.852238	51.521677
3385.420444	394486.974970	51.526682
3384.740483	394195.589265	51.531687
3383.976362	393927.198540	51.536692
3383.526646	393646.526523	51.541697
3382.494630	393392.386647	51.546701
3382.355333	393104.211526	51.551706
3381.466057	392829.018033	51.556711
3380.624052	392570.367164	51.561716
3380.559639	392264.451383	51.566721
3378.942802	392016.801329	51.571725
3378.908658	391715.401850	51.576730
3378.096682	391438.990148	51.581735
3377.250950	391189.178182	51.586740
3376.926884	390897.632344	51.591745
3376.024021	390627.356599	51.596749
3375.381221	390365.403321	51.601754
3374.653404	390096.265519	51.606759
3373.905395	389816.805152	51.611764
3373.363324	389543.921339	51.616769
3372.439724	389278.037703	51.621773
3371.780810	389032.351298	51.626778
3371.276314	388742.850669	51.631783
3370.388638	388462.232128	51.636788
3369.774048	388194.740473	51.641793
3368.920135	387945.466587	51.646797
3368.398887	387676.964615	51.651802
3367.522655	387410.525739	51.656807
3366.813182	387130.682481	51.661812
3366.736811	386879.447404	51.666817
3365.713285	386607.660254	51.671821
3364.845996	386332.743887	51.676826
3363.972645	386076.467001	51.681831
3363.448337	385811.384981	51.686836
3362.816460	385542.452581	51.691841
3362.377393	385289.255001	51.696845
3362.000179	385018.523797	51.701850
3361.073343	384753.294441	51.706855
3360.302515	384488.420007	51.711860
3359.959688	384220.373339	51.716865
3359.071845	383961.566457	51.721869
3358.280530	383693.129185	51.726874
3357.499705	383425.807369	51.731879
3356.840474	383158.718761	51.736884
3356.431832	382897.870516	51.741889
3355.205307	382631.630899	51.746893
3354.956629	382370.168790	51.751898
3353.807397	382119.046022	51.756903
3353.584993	381854.295355	51.761908
3353.117673	381579.764250	51.766913
3351.969828	381320.904249	51.771917
3351.292421	381075.117433	51.776922
3350.800458	380807.095807	51.781927
3350.010382	380546.953219	51.786932
3349.473544	380282.724774	51.791937
3348.833643	380033.644404	51.796941
3348.216447	379767.797374	51.801946
3347.319517	379511.581738	51.806951
3346.612275	379256.911408	51.811956
3346.300241	378984.474008	51.816961
3344.965553	378733.104367	51.821965
3344.397437	378479.170082	51.826970
3343.836667	378218.517981	51.831975
3343.388435	377960.466272	51.836980
3342.824504	377696.428283	51.841985
3341.993736	377451.457048	51.846989
3341.175357	377183.945725	51.851994
3340.356746	376927.497560	51.856999
3339.766468	376680.117993	51.862004
3339.080668	376415.073399	51.867009
3338.038640	376181.803381	51.872013
3337.646140	375928.105001	51.877018
3336.741164	375673.519473	51.882023
3336.275162	375422.932930	51.887028
3335.618690	375180.209772	51.892033
3335.310403	374933.003935	51.897037
3334.613738	374675.657419	51.902042
3333.763074	374415.611775	51.907047
3333.203475	374163.353450	51.912052
3332.764611	373916.365687	51.917057
3331.778673	373673.736659	51.922061
3331.059475	373405.879696	51.927066
3330.803166	373143.518926	51.932071
3329.713098	372889.377993	51.937076
3328.873434	372636.645954	51.942081
3327.890670	372399.961817	51.947085
3327.730450	372134.272441	51.952090
3327.174746	371890.013255	51.957095
3326.367529	371651.719913	51.962100
3325.881779	371378.267277	51.967105
3324.981859	371123.729513	51.972109
3324.473721	370874.140001	51.977114
3323.924861	370626.463507	51.982119
3323.005914	370374.977158	51.987124
3322.329854	370116.124007	51.992129
3321.540345	369885.043209	51.997133
3321.182541	369617.283331	52.002138
3320.326181	369344.639632	52.007143
3319.471481	369143.127806	52.012148
3319.074858	368860.562602	52.017153
3318.585475	368615.333051	52.022157
3317.771693	368371.985243	52.027162
3317.471017	368112.094055	52.032167
3316.255666	367856.035098	52.037172
3315.820453	367618.118738	52.042177
3314.975712	367355.001682	52.047181
3314.466879	367117.246942	52.052186
3314.056485	366865.023987	52.057191
3313.028658	366615.645082	52.062196
3312.349569	366345.753571	52.067201
3311.415959	366112.233322	52.072205
3310.896631	365853.279529	52.077210
3310.165980	365612.447859	52.082215
3309.399599	365352.130901	52.087220
3308.921404	365112.681487	52.092225
3308.359018	364869.274919	52.097229
3307.624238	364620.881889	52.102234
3307.265625	364373.318559	52.107239
3306.073830	364131.457939	52.112244
3305.587583	363877.805552	52.117249
3304.898865	363641.460533	52.122253
3304.319938	363398.608599	52.127258
3303.433225	363140.079291	52.132263
3302.862268	362880.760711	52.137268
3302.392679	362640.279352	52.142273
3301.190684	362385.637932	52.147277
3300.547482	362162.178884	52.152282
3300.523432	361891.648808	52.157287
3299.510670	361686.973723	52.162292
3298.893288	361409.308243	52.167297
3298.122486	361186.653599	52.172301
3297.250938	360920.959511	52.177306
3296.765149	360708.843032	52.182311
3296.402861	360439.859541	52.187316
3295.768320	360183.818854	52.192321
3294.658181	359977.625099	52.197325
3293.827234	359712.121498	52.202330
3293.477439	359459.467223	52.207335
3292.917616	359244.404234	52.212340
3292.590254	358970.979357	52.217345
3291.575689	358751.532932	52.222349
3291.232407	358482.103029	52.227354
3290.206619	358245.072164	52.232359
3289.484554	358012.852569	52.237364
3288.980029	357733.545075	52.242369
3288.294370	357497.143924	52.247373
3287.523669	357248.031235	52.252378
3287.043637	357017.829992	52.257383
3286.181926	356760.026107	52.262388
3285.718517	356531.703164	52.267393
3284.695675	356270.155944	52.272397
3284.385333	356047.125287	52.277402
3283.534852	355783.665122	52.282407
3282.974703	355545.275449	52.287412
3282.689676	355289.561464	52.292417
3281.690804	355035.155217	52.297421
3280.510750	354802.357103	52.302426
3280.424807	354541.976206	52.307431
3279.618751	354298.707987	52.312436
3279.292303	354051.036380	52.317441
3278.279762	353807.951227	52.322445
3277.565127	353550.133417	52.327450
3276.994941	353315.679765	52.332455
3276.010889	353077.905712	52.337460
3275.835987	352813.916420	52.342465
3274.642253	352583.070242	52.347469
3273.830678	352345.087469	52.352474
3273.451055	352106.297249	52.357479
3272.762691	351845.845617	52.362484
3271.988661	351634.042194	52.367489
3271.147564	351379.796935	52.372493
3270.868941	351148.418065	52.377498
3270.314973	350901.404047	52.382503
3269.056522	350659.870495	52.387508
3268.698876	350419.898603	52.392513
3267.926232	350191.571590	52.397517
3267.369608	349949.236702	52.402522
3267.127538	349709.676096	52.407527
3266.345585	349462.131726	52.412532
3265.409258	349213.847121	52.417537
3264.516285	348992.991514	52.422541
3264.056903	348736.713851	52.427546
3263.367308	348502.131042	52.432551
3262.447700	348271.961391	52.437556
3262.473155	348030.315095	52.442561
3261.486321	347793.816541	52.447565
3260.924113	347533.579120	52.452570
3259.937353	347311.459141	52.457575
3259.447706	347072.766387	52.462580
3258.896860	346818.607081	52.467585
3257.909844	346586.837760	52.472589
3257.377772	346341.989106	52.477594
3256.859980	346106.962021	52.482599
3255.715406	345873.025808	52.487604
3255.555385	345612.996076	52.492609
3254.458989	345392.260539	52.497613
3253.846506	345154.164747	52.502618
3253.254116	344925.889876	52.507623
3252.258034	344694.725363	52.512628
3252.200290	344446.433877	52.517633
3251.020219	344216.034764	52.522637
3250.572873	343975.591820	52.527642
3249.734125	343755.165786	52.532647
3248.877868	343521.021943	52.537652
3248.710360	343270.477531	52.542657
3247.669525	343034.222845	52.547661
3246.928177	342799.599856	52.552666
3246.261175	342570.589653	52.557671
3245.489422	342332.991502	52.562676
3245.305581	342115.383199	52.567681
3244.535670	341876.892081	52.572685
3243.711277	341642.965089	52.577690
3243.245922	341409.107693	52.582695
3242.593289	341181.006442	52.587700
3241.763582	340940.688424	52.592705
3241.205622	340713.817799	52.597709
3240.517741	340478.133893	52.602714
3240.015035	340253.722043	52.607719
3239.303149	340020.458500	52.612724
3238.944382	339758.475164	52.617729
3238.026527	339536.035634	52.622733
3237.273719	339301.274048	52.627738
3236.585804	339063.166611	52.632743
3235.838265	338829.242519	52.637748
3235.291476	338599.333349	52.642753
3234.868667	338360.825008	52.647757
3233.919868	338118.656930	52.652762
3233.260645	337879.878761	52.657767
3232.574544	337662.334693	52.662772
3232.079402	337408.916836	52.667777
3231.311328	337189.805876	52.672781
3230.613494	336949.808540	52.677786
3230.240966	336714.392027	52.682791
3229.338130	336484.404540	52.687796
3228.771645	336239.114297	52.692801
3228.013965	336004.290831	52.697805
3227.295827	335773.711650	52.702810
3226.580967	335540.687271	52.707815
3225.837681	335304.204392	52.712820
3225.693355	335063.909151	52.717825
3224.804784	334836.892371	52.722829
3223.891965	334586.253992	52.727834
3223.632179	334354.884732	52.732839
3222.790091	334122.868552	52.737844
3222.282360	333879.800894	52.742849
3221.504240	333647.722107	52.747853
3220.625424	333409.752217	52.752858
3219.715143	333166.643959	52.757863
3219.120961	332938.250643	52.762868
3218.632720	332704.671799	52.767873
3217.453304	332487.036668	52.772877
3217.027864	332251.384287	52.777882
3216.439918	332013.567412	52.782887
3215.403418	331797.002315	52.787892
3215.271192	331571.739385	52.792897
3214.369195	331341.302116	52.797901
3213.902643	331106.339931	52.802906
3213.342732	330878.265688	52.807911
3212.611951	330650.650581	52.812916
3212.156423	330414.717019	52.817921
3211.446544	330186.257040	52.822925
3210.622235	329946.943360	52.827930
3210.314015	329708.540186	52.832935
3209.070511	329480.620764	52.837940
3208.518747	329244.647853	52.842945
3208.075049	329022.889026	52.847949
3207.001435	328787.226404	52.852954
3206.560840	328550.088088	52.857959
3205.794372	328328.200111	52.862964
3205.373885	328083.241025	52.867969
3204.489548	327862.643368	52.872973
3203.684791	327639.690177	52.877978
3203.569136	327395.648200	52.882983
3202.761691	327181.808864	52.887988
3202.053301	326929.813815	52.892993
3201.674781	326708.063586	52.897997
3200.812985	326473.480779	52.903002
3200.619174	326226.519654	52.908007
3199.231091	325995.252207	52.913012
3198.950724	325759.353238	52.918017
3198.100202	325531.614838	52.923021
3197.621294	325282.175354	52.928026
3196.936119	325054.791388	52.933031
3196.265519	324819.791679	52.938036
3195.752341	324588.967465	52.943041
3195.018215	324352.779828	52.948045
3194.415926	324111.121987	52.953050
3193.460826	323867.736991	52.958055
3192.546426	323638.144874	52.963060
3192.089679	323396.665666	52.968065
3191.529419	323163.655349	52.973069
3190.820640	322927.459754	52.978074
3190.422150	322690.145037	52.983079
3189.667023	322459.429739	52.988084
3189.085805	322225.503607	52.993089
3188.062568	321992.385180	52.998093
3187.581029	321745.125503	53.003098
3187.075806	321506.093081	53.008103
3186.090159	321278.288372	53.013108
3185.741184	321045.824650	53.018113
3185.113687	320799.069238	53.023117
3184.177026	320571.254998	53.028122
3183.368696	320335.093737	53.033127
3182.830572	320107.597221	53.038132
3182.139589	319858.990575	53.043137
3181.384560	319634.506310	53.048141
3180.870117	319406.978868	53.053146
3180.396562	319170.939914	53.058151
3179.426625	318931.999783	53.063156
3178.930568	318694.231742	53.068161
3178.069755	318469.761444	53.073165
3177.220598	318229.527306	53.078170
3176.813997	317993.907713	53.083175
3176.057937	317774.817348	53.088180
3175.488983	317545.689937	53.093185
3174.776678	317311.237434	53.098189
3174.229108	317072.353193	53.103194
3173.440164	316840.254304	53.108199
3172.650778	316608.205872	53.113204
3172.283983	316372.652495	53.118209
3171.477296	316136.658904	53.123213
3170.859140	315902.290054	53.128218
3170.459455	315671.323664	53.133223
3169.566875	315437.888392	53.138228
3168.845244	315210.715044	53.143233
3168.131364	314978.090758	53.148237
3167.588568	314740.829957	53.153242
3166.800988	314501.086443	53.158247
3165.906156	314284.938827	53.163252
3165.746708	314049.551067	53.168257
3165.085926	313818.851080	53.173261
3164.316869	313579.357202	53.178266
3163.595823	313344.438720	53.183271
3163.124654	313108.690808	53.188276
3162.243267	312870.333565	53.193281
3161.233940	312641.672439	53.198285
3161.067035	312408.803269	53.203290
3160.233437	312177.261390	53.208295
3159.361163	311949.646661	53.213300
3158.966448	311710.598795	53.218305
3158.277111	311493.063566	53.223309
3157.283605	311250.544465	53.228314
3156.885725	311008.134323	53.233319
3156.121087	310789.692961	53.238324
3155.653888	310564.328674	53.243329
3154.907867	310335.290230	53.248333
3154.209058	310095.064853	53.253338
3153.662667	309859.602255	53.258343
3152.501568	309637.274461	53.263348
3152.255778	309393.232667	53.268353
3151.529765	309165.971370	53.273357
3150.558419	308938.366498	53.278362
3150.080841	308703.629262	53.283367
3149.373966	308489.503648	53.288372
3148.960065	308246.912234	53.293377
3147.843194	308029.922223	53.298381
3147.286163	307797.436802	53.303386
3146.695116	307555.534195	53.308391
3145.740330	307343.126584	53.313396
3145.416215	307122.266197	53.318401
3145.253254	306891.652157	53.323405
3144.491980	306653.161708	53.328410
3143.524865	306421.757340	53.333415
3142.733288	306199.034004	53.338420
3142.048468	305967.278596	53.343425
3141.287310	305735.560338	53.348429
3141.005716	305515.658261	53.353434
3140.446122	305287.116023	53.358439
3139.424745	305055.030346	53.363444
3139.066879	304819.987124	53.368449
3138.283245	304588.423304	53.373453
3137.486854	304362.998397	53.378458
3137.299757	304128.767384	53.383463
3136.226859	303881.153745	53.388468
3135.864834	303651.176988	53.393473
3134.979799	303431.265315	53.398477
3134.071174	303190.551276	53.403482
3133.685800	302956.375236	53.408487
3132.908359	302731.199489	53.413492
3132.232917	302507.331510	53.418497
3131.898735	302281.066311	53.423501
3130.876992	302041.488866	53.428506
3130.193680	301800.660584	53.433511
3129.388899	301586.157875	53.438516
3128.881300	301350.572631	53.443521
3127.998763	301126.964650	53.448525
3127.521912	300903.241229	53.453530
3126.882681	300672.947381	53.458535
3126.121098	300442.672573	53.463540
3125.500002	300209.421095	53.468545
3124.620714	299995.386484	53.473549
3124.003585	299763.050557	53.478554
3123.673091	299534.387086	53.483559
3122.743777	299305.690740	53.488564
3122.419345	299096.125740	53.493569
3121.617431	298860.405307	53.498573
3120.551918	298631.373103	53.503578
3120.124868	298389.429768	53.508583
3119.591847	298172.333050	53.513588
3119.035467	297947.905312	53.518593
3118.434561	297712.406246	53.523597
3117.585693	297492.582820	53.528602
3117.092659	297251.361513	53.533607
3116.031230	297035.060170	53.538612
3115.743767	296799.051963	53.543617
3115.195179	296577.932087	53.548621
3114.146209	296348.436077	53.553626
3113.609257	296110.327294	53.558631
3112.849957	295884.910586	53.563636
3112.355068	295654.078213	53.568641
3111.762748	295435.790862	53.573645
3111.081574	295199.461081	53.578650
3110.716920	294962.316929	53.583655
3109.417954	294739.098170	53.588660
3109.052905	294510.103112	53.593665
3108.321576	294267.489820	53.598669
3107.748368	294049.809255	53.603674
3107.466452	293818.635601	53.608679
3106.515435	293592.253603	53.613684
3105.661526	293353.198700	53.618689
3105.172943	293132.345908	53.623693
3104.382617	292894.350110	53.628698
3104.126772	292672.696035	53.633703
3102.807750	292436.005894	53.638708
3102.584665	292199.906115	53.643713
3102.093067	291971.081400	53.648717
3101.310785	291747.319599	53.653722
3100.483729	291505.966558	53.658727
3099.606230	291273.203877	53.663732
3099.257800	291047.360872	53.668737
3098.466120	290819.652280	53.673741
3097.629203	290585.736535	53.678746
3097.256938	290345.762141	53.683751
3096.354564	290130.626096	53.688756
3095.697241	289897.267116	53.693761
3095.062135	289663.547885	53.698765
3094.112744	289432.985280	53.703770
3093.849819	289205.777486	53.708775
3093.119724	288980.935564	53.713780
3092.607467	288734.487715	53.718785
3091.555743	288519.552432	53.723789
3091.249333	288292.911152	53.728794
3090.586218	288045.136854	53.733799
3089.755248	287836.227554	53.738804
3089.289876	287597.921176	53.743809
3088.650778	287370.313211	53.748813
3087.954044	287141.466291	53.753818
3087.090638	286910.124271	53.758823
3086.354356	286681.538003	53.763828
3085.626457	286454.707564	53.768833
3084.982928	286228.194724	53.773837
3084.354946	286008.912225	53.778842
3083.704120	285766.457266	53.783847
3083.186143	285548.226769	53.788852
3082.703582	285312.774111	53.793857
3081.715448	285091.459744	53.798861
3081.199843	284857.718434	53.803866
3080.576681	284632.423985	53.808871
3079.815365	284395.359533	53.813876
3079.417810	284164.298818	53.818881
3078.352473	283937.520464	53.823885
3077.654405	283708.289872	53.828890
3077.392125	283487.725805	53.833895
3076.478765	283255.574778	53.838900
3076.055302	283026.733394	53.843905
3075.307409	282802.043651	53.848909
3074.365673	282566.433154	53.853914
3073.657862	282339.444752	53.858919
3073.152984	282120.293845	53.863924
3072.744839	281873.290727	53.868929
3071.850937	281650.661146	53.873933
3071.334637	281409.889242	53.878938
3070.761625	281182.191475	53.883943
3069.917292	280962.992061	53.888948
3069.696796	280721.867505	53.893953
3068.827431	280495.387989	53.898957
3067.813546	280262.411396	53.903962
3067.767768	280025.384866	53.908967
3066.714885	279798.755948	53.913972
3066.173405	279552.842905	53.918977
3065.050918	279332.464650	53.923981
3064.517579	279102.493412	53.928986
3064.482615	278854.742739	53.933991
3063.662507	278632.202630	53.938996
3062.844458	278404.670362	53.944001
3061.915159	278170.482954	53.949005
3061.369443	277930.402547	53.954010
3061.065637	277699.987275	53.959015
3060.170936	277464.902915	53.964020
3059.761365	277235.854162	53.969025
3059.067609	276997.146915	53.974029
3057.850395	276760.891063	53.979034
3057.682622	276519.069799	53.984039
3056.637712	276303.747140	53.989044
3056.233446	276069.196316	53.994049
3055.463564	275835.340066	53.999053
3054.441098	275597.346979	54.004058
3054.032196	275376.116859	54.009063
3053.119367	275159.168787	54.014068
3052.838133	274907.789369	54.019073
3052.192703	274697.038751	54.024077
3051.295283	274463.049925	54.029082
3050.694431	274223.080044	54.034087
3050.044650	273996.336020	54.039092
3049.262087	273767.320883	54.044097
3048.513631	273536.874145	54.049101
3047.672576	273316.120075	54.054106
3047.286668	273080.191252	54.059111
3046.312473	272866.513058	54.064116
3046.032384	272632.273942	54.069121
3045.612334	272410.409174	54.074125
3044.454526	272172.285071	54.079130
3044.072353	271950.185182	54.084135
3043.371553	271710.384340	54.089140
3042.115505	271484.882772	54.094145
3041.950617	271269.523220	54.099149
3041.086260	271044.596472	54.104154
3040.587831	270819.077029	54.109159
3039.700316	270604.137644	54.114164
3039.428581	270361.671494	54.119169
3038.333317	270142.537386	54.124173
3037.437055	269928.949401	54.129178
3037.551199	269689.554999	54.134183
3036.646628	269473.498050	54.139188
3035.775998	269246.841008	54.144193
3035.478739	269032.394456	54.149197
3034.783293	268790.225161	54.154202
3034.264777	268569.446741	54.159207
3033.344643	268348.757446	54.164212
3032.581811	268111.387135	54.169217
3031.960648	267887.925610	54.174221
3031.318610	267663.448758	54.179226
3030.983536	267429.092705	54.184231
3030.049737	267210.316177	54.189236
3029.592058	266968.976012	54.194241
3028.919406	266745.701440	54.199245
3028.299686	266515.695017	54.204250
3027.886100	266281.020891	54.209255
3026.536954	266056.835028	54.214260
3026.175276	265818.867558	54.219265
3025.685231	265591.438857	54.224269
3024.831834	265364.551693	54.229274
3024.137714	265139.320341	54.234279
3023.582668	264906.172021	54.239284
3022.727113	264685.092312	54.244289
3022.203744	264449.163254	54.249293
3021.295973	264227.480859	54.254298
3020.908305	263988.117920	54.259303
3020.442647	263759.565897	54.264308
3019.632220	263538.581639	54.269313
3018.871160	263298.055832	54.274317
3018.103997	263083.737622	54.279322
3017.688415	262843.997909	54.284327
3016.794971	262616.991539	54.289332
3016.252052	262379.971931	54.294337
3015.787927	262154.782566	54.299341
3014.914482	261933.911284	54.304346
3014.435697	261697.671568	54.309351
3013.689629	261465.880274	54.314356
3013.246821	261234.779729	54.319361
3012.540037	260993.075661	54.324365
3011.526292	260766.981149	54.329370
3011.020180	260521.323710	54.334375
3010.465521	260288.331598	54.339380
3009.583996	260051.520357	54.344385
3008.581047	259836.732554	54.349389
3008.228962	259610.712573	54.354394
3007.899715	259367.040171	54.359399
3006.842635	259152.057781	54.364404
3006.286595	258916.800540	54.369409
3006.019381	258674.570655	54.374413
3004.598577	258449.510416	54.379418
3004.267684	258211.493215	54.384423
3003.698055	257993.709696	54.389428
3002.836316	257761.532625	54.394433
3002.299354	257535.696684	54.399437
3001.374167	257308.649062	54.404442
3000.943405	257075.080181	54.409447
3000.518136	256858.930293	54.414452
2999.869615	256627.637486	54.419457
2999.197240	256384.786593	54.424461
2998.241789	256169.740022	54.429466
2997.642702	255933.244849	54.434471
2997.090829	255699.289187	54.439476
2996.313600	255463.433971	54.444481
2996.148556	255239.069637	54.449485
2995.038869	255004.795616	54.454490
2994.566710	254770.599222	54.459495
2993.940872	254543.914731	54.464500
2993.264659	254306.313161	54.469505
2992.749133	254067.540441	54.474509
2991.611754	253843.891928	54.479514
2990.862639	253606.302786	54.484519
2990.294150	253386.282930	54.489524
2989.860886	253152.820936	54.494529
2989.024461	252924.516417	54.499533
2988.008671	252692.446045	54.504538
2987.917405	252463.030956	54.509543
2987.251860	252242.594943	54.514548
2986.335015	252005.620222	54.519553
2985.873999	251775.322313	54.524557
2984.994813	251542.187729	54.529562
2984.449062	251316.640639	54.534567
2983.665746	251091.411594	54.539572
2983.190551	250849.351690	54.544577
2982.740859	250627.024575	54.549581
2981.645279	250404.850947	54.554586
2981.329968	250155.916313	54.559591
2980.453249	249934.167086	54.564596
2979.912843	249704.954247	54.569601
2979.581737	249462.389775	54.574605
2978.447354	249239.434481	54.579610
2977.918104	249002.122669	54.584615
2977.324892	248775.746314	54.589620
2976.809616	248536.726789	54.594625
2976.101192	248309.197937	54.599629
2975.322306	248070.450087	54.604634
2974.607611	247832.354578	54.609639
2973.547512	247611.147104	54.614644
2972.852713	247381.834922	54.619649
2972.787480	247153.187414	54.624653
2971.861641	246923.759749	54.629658
2971.282198	246692.265824	54.634663
2970.407979	246459.953115	54.639668
2970.112665	246227.854733	54.644673
2968.960687	245992.174384	54.649677
2968.059272	245774.739056	54.654682
2967.822221	245542.861802	54.659687
2967.064637	245314.607058	54.664692
2966.244795	245087.814090	54.669697
2965.248330	244858.171881	54.674701
2964.978822	244642.853842	54.679706
2964.503872	244421.278749	54.684711
2963.728332	244193.283442	54.689716
2963.154083	243964.034340	54.694721
2962.760735	243736.183059	54.699725
2961.647710	243503.098444	54.704730
2961.418197	243276.775424	54.709735
2960.533187	243053.408673	54.714740
2959.667287	242821.177479	54.719745
2959.126619	242596.305531	54.724749
2958.563705	242371.259262	54.729754
2958.161026	242138.752303	54.734759
2957.004636	241913.087824	54.739764
2956.557861	241675.241130	54.744769
2955.964745	241444.522729	54.749773
2955.099078	241237.097161	54.754778
2954.828948	240985.753076	54.759783
2954.390352	240760.002614	54.764788
2953.115534	240535.632741	54.769793
2952.581343	240293.473715	54.774797
2952.009032	240070.801503	54.779802
2951.446668	239842.475063	54.784807
2950.686019	239617.796407	54.789812
2950.090413	239378.984874	54.794817
2949.863027	239148.238631	54.799821
2949.062991	238916.743212	54.804826
2948.387049	238676.061560	54.809831
2947.819666	238442.824209	54.814836
2946.740156	238213.157003	54.819841
2946.094385	237970.078515	54.824845
2945.341273	237744.078362	54.829850
2944.840378	237509.890333	54.834855
2944.200927	237287.998287	54.839860
2943.480452	237052.725624	54.844865
2943.247663	236810.119136	54.849869
2942.116648	236580.132579	54.854874
2941.622090	236343.272465	54.859879
2940.768391	236117.266268	54.864884
2940.076097	235885.760378	54.869889
2939.728329	235649.235109	54.874893
2938.859463	235422.392560	54.879898
2938.430521	235176.485289	54.884903
2937.465319	234958.851266	54.889908
2936.739030	234707.364862	54.894913
2936.420355	234475.090093	54.899917
2935.816681	234253.657306	54.904922
2935.192381	234012.036171	54.909927
2934.402513	233776.603864	54.914932
2933.604377	233536.768371	54.919937
2932.861651	233307.720908	54.924941
2931.748302	233075.600761	54.929946
2931.573109	232843.027089	54.934951
2931.035126	232605.546226	54.939956
2930.044590	232369.308888	54.944961
2929.785794	232141.078806	54.949965
2929.062183	231918.244513	54.954970
2928.456722	231680.140120	54.959975
2927.615514	231440.393157	54.964980
2927.150236	231202.573348	54.969985
2926.586492	230971.542671	54.974989
2925.669486	230740.644899	54.979994
2925.241429	230501.649774	54.984999
2924.064762	230277.134336	54.990004
2923.250236	230034.025891	54.995009
2923.226165	229808.387047	55.000013
2922.476757	229572.016929	55.005018
2921.890865	229336.945559	55.010023
2921.003770	229101.566048	55.015028
2920.363455	228865.537021	55.020033
2919.789407	228626.340922	55.025037
2918.921481	228398.955174	55.030042
2918.502863	228154.490730	55.035047
2917.738499	227928.286512	55.040052
2916.791459	227695.339147	55.045057
2916.657871	227441.818363	55.050061
2915.953262	227217.936269	55.055066
2915.320075	226981.822204	55.060071
2914.586131	226747.201492	55.065076
2913.870737	226505.182139	55.070081
2913.310434	226271.566440	55.075085
2912.574076	226043.135065	55.080090
2912.356650	225788.066763	55.085095
2911.612981	225559.434212	55.090100
2910.545627	225316.926696	55.095105
2909.859061	225073.926788	55.100109
2909.050454	224837.706644	55.105114
2908.468814	224596.944802	55.110119
2907.803096	224358.131971	55.115124
2907.147699	224119.369144	55.120129
2906.828359	223888.904702	55.125133
2905.927408	223650.882327	55.130138
2905.457197	223414.434631	55.135143
2904.726129	223178.703641	55.140148
2903.662072	222951.376868	55.145153
2903.339207	222701.185251	55.150157
2902.687423	222470.166626	55.155162
2902.207457	222224.062235	55.160167
2901.102615	221996.477429	55.165172
2900.558067	221757.920744	55.170177
2899.811033	221518.836774	55.175181
2899.148447	221294.811991	55.180186
2898.717053	221051.033242	55.185191
2898.116073	220817.720316	55.190196
2897.238939	220581.358598	55.195201
2896.821287	220334.334021	55.200205
2896.008481	220102.126167	55.205210
2895.276429	219859.837374	55.210215
2895.000864	219624.580036	55.215220
2894.164098	219372.253323	55.220225
2893.753384	219138.571929	55.225229
2892.908688	218903.292496	55.230234
2892.547380	218654.342609	55.235239
2891.520538	218414.091091	55.240244
2890.555997	218181.684323	55.245249
2890.185594	217931.478235	55.250253
2889.540059	217689.870441	55.255258
2888.564024	217451.701696	55.260263
2887.401990	217213.779607	55.265268
2887.267670	216982.174551	55.270273
2886.362427	216745.269893	55.275277
2885.884539	216518.099485	55.280282
2885.290518	216276.246603	55.285287
2884.617417	216043.215305	55.290292
2884.423450	215804.164683	55.295297
2883.579568	215571.531170	55.300301
2882.539838	215330.872335	55.305306
2882.029531	215097.665763	55.310311
2881.355970	214864.740420	55.315316
2880.846691	214617.445015	55.320321
2880.212695	214386.666166	55.325325
2879.369931	214153.019133	55.330330
2878.803646	213909.337490	55.335335
2878.311947	213673.052735	55.340340
2877.580068	213436.972328	55.345345
2876.845281	213192.136314	55.350349
2875.894244	212950.135632	55.355354
2875.308283	212709.961783	55.360359
2874.660502	212486.955881	55.365364
2874.317479	212249.927258	55.370369
2873.740695	212004.014307	55.375373
2872.774669	211772.228159	55.380378
2872.165208	211527.556815	55.385383
2871.532343	211294.523242	55.390388
2870.738500	211051.448443	55.395393
2870.271554	210815.348455	55.400397
2869.814492	210579.324155	55.405402
2869.215727	210335.406674	55.410407
2867.993009	210091.308951	55.415412
2867.441377	209847.475011	55.420417
2867.259059	209608.407219	55.425421
2866.131049	209371.959211	55.430426
2865.527407	209133.583622	55.435431
2864.712133	208887.313423	55.440436
2864.237465	208664.840983	55.445441
2863.822186	208423.867453	55.450445
2863.220364	208185.266202	55.455450
2862.599657	207927.005653	55.460455
2861.846633	207696.804655	55.465460
2861.097080	207453.202557	55.470465
2860.422378	207201.533499	55.475469
2859.455398	206964.483982	55.480474
2858.932355	206725.061569	55.485479
2858.775163	206495.610830	55.490484
2857.867900	206255.882094	55.495489
2857.247818	206006.131206	55.500493
2856.314590	205766.892196	55.505498
2855.729614	205518.512303	55.510503
2855.288375	205283.078951	55.515508
2854.400656	205040.743203	55.520513
2854.051241	204790.331090	55.525517
2852.887425	204551.922657	55.530522
2852.341712	204314.931753	55.535527
2851.823408	204070.899919	55.540532
2851.098583	203827.563597	55.545537
2850.459537	203592.193977	55.550541
2849.603741	203353.589078	55.555546
2848.952048	203107.304570	55.560551
2848.446568	202874.589248	55.565556
2847.634647	202639.123739	55.570561
2847.049035	202398.685776	55.575565
2846.346799	202160.672488	55.580570
2845.719300	201918.512541	55.585575
2845.406384	201683.697425	55.590580
2844.611631	201439.809932	55.595585
2843.902300	201190.005357	55.600589
2843.333168	200957.231833	55.605594
2842.645057	200711.650941	55.610599
2841.977499	200471.921562	55.615604
2841.106197	200236.233978	55.620609
2840.615292	199981.501134	55.625613
2839.916055	199742.149047	55.630618
2839.108113	199492.609702	55.635623
2838.363730	199252.719774	55.640628
2837.701659	199012.245265	55.645633
2837.400372	198781.169340	55.650637
2836.414856	198544.323887	55.655642
2835.837310	198288.009526	55.660647
2835.109225	198042.269084	55.665652
2834.526419	197812.743512	55.670657
2834.072076	197570.995661	55.675661
2833.228518	197324.716996	55.680666
2832.443046	197081.331492	55.685671
2832.218376	196847.032659	55.690676
2831.575476	196602.023547	55.695681
2830.924579	196349.076872	55.700685
2829.939474	196107.941618	55.705690
2829.344383	195859.467473	55.710695
2828.849624	195622.583089	55.715700
2827.575184	195376.700105	55.720705
2827.533597	195131.424675	55.725709
2826.655905	194899.337664	55.730714
2825.997740	194655.574560	55.735719
2825.429162	194410.844160	55.740724
2824.756324	194161.118291	55.745729
2823.983555	193914.259615	55.750733
2823.563953	193683.263548	55.755738
2822.916817	193430.343631	55.760743
2822.340868	193174.245567	55.765748
2821.263144	192945.074858	55.770753
2821.035383	192699.217421	55.775757
2819.989662	192451.035155	55.780762
2819.501014	192206.850098	55.785767
2819.142505	191961.042525	55.790772
2818.013861	191711.922913	55.795777
2817.368011	191462.753563	55.800781
2816.852002	191221.186032	55.805786
2816.342869	190979.860360	55.810791
2815.507512	190738.931085	55.815796
2814.414979	190499.087028	55.820801
2813.976051	190246.048914	55.825805
2813.397563	190013.937668	55.830810
2812.656956	189751.700549	55.835815
2812.183645	189519.435114	55.840820
2811.323593	189277.117671	55.845825
2810.919710	189025.530891	55.850829
2810.074909	188788.951373	55.855834
2809.358877	188554.070169	55.860839
2808.989313	188310.038856	55.865844
2808.156284	188063.168845	55.870849
2807.500699	187808.168051	55.875853
2806.707246	187584.079644	55.880858
2806.187998	187329.963159	55.885863
2805.262768	187083.698191	55.890868
2804.457266	186845.303129	55.895873
2804.073862	186598.458796	55.900877
2803.291057	186358.904992	55.905882
2802.719458	186121.468954	55.910887
2802.083887	185881.321870	55.915892
2801.273037	185640.415086	55.920897
2800.668543	185403.331501	55.925901
2800.022054	185161.574346	55.930906
2799.434749	184921.017641	55.935911
2798.717707	184687.784772	55.940916
2798.159586	184440.623698	55.945921
2797.807913	184197.133136	55.950925
2797.092528	183959.527751	55.955930
2796.430353	183707.108002	55.960935
2795.801207	183462.304278	55.965940
2794.665864	183215.572199	55.970945
2794.309418	182982.469271	55.975949
2793.783020	182734.282320	55.980954
2793.096428	182482.547658	55.985959
2792.438651	182242.932559	55.990964
2791.469741	182005.390614	55.995969
2791.207710	181743.302115	56.000973
2790.227577	181506.489743	56.005978
2789.619043	181259.341844	56.010983
2788.990195	181014.780777	56.015988
2788.244815	180768.204342	56.020993
2787.923721	180520.430037	56.025997
2786.888125	180281.229116	56.031002
2786.162357	180031.906308	56.036007
2785.647962	179790.666724	56.041012
2785.105766	179544.561252	56.046017
2784.419723	179297.729535	56.051021
2783.765683	179063.194043	56.056026
2783.157471	178814.368569	56.061031
2782.794378	178560.710512	56.066036
2781.636820	178319.657535	56.071041
2781.003033	178072.633950	56.076045
2780.453333	177834.807228	56.081050
2779.920112	177578.282104	56.086055
2779.432185	177326.444729	56.091060
2778.780827	177086.018274	56.096065
2778.470090	176833.888734	56.101069
2777.501822	176583.670966	56.106074
2776.882221	176322.715735	56.111079
2775.916214	176070.974487	56.116084
2774.984309	175825.219853	56.121089
2774.518974	175572.397606	56.126093
2773.595270	175332.406142	56.131098
2773.405180	175087.975647	56.136103
2772.443126	174845.958202	56.141108
2771.847500	174603.235537	56.146113
2771.078623	174340.459832	56.151117
2770.429473	174093.640764	56.156122
2769.843046	173843.264965	56.161127
2769.333730	173603.243610	56.166132
2768.596195	173354.408245	56.171137
2768.091559	173104.799916	56.176141
2767.151731	172859.255440	56.181146
2766.725153	172603.533425	56.186151
2765.899938	172349.745685	56.191156
2765.231136	172110.203753	56.196161
2765.051228	171866.045746	56.201165
2763.848728	171616.328474	56.206170
2763.315612	171361.674235	56.211175
2762.732402	171125.914490	56.216180
2762.207486	170869.494491	56.221185
2761.406458	170614.200864	56.226189
2760.452283	170372.947155	56.231194
2760.366277	170117.467242	56.236199
2759.434823	169863.102131	56.241204
2758.471886	169626.381628	56.246209
2758.143096	169366.646946	56.251213
2757.195767	169128.223035	56.256218
2756.602826	168884.085693	56.261223
2756.094094	168627.004119	56.266228
2755.321693	168387.298226	56.271233
2754.919120	168136.014464	56.276237
2753.802109	167891.000103	56.281242
2753.266892	167628.970248	56.286247
2752.553256	167389.210517	56.291252
2751.761878	167153.241219	56.296257
2751.581789	166907.538071	56.301261
2750.754237	166591.710825	56.306266
2749.788647	166356.003038	56.311271
2749.574857	166079.310281	56.316276
2748.922193	165863.722702	56.321281
2748.177618	165572.546029	56.326285
2747.283655	165370.541286	56.331290
2747.011240	165091.233164	56.336295
2746.497277	164835.271992	56.341300
2745.469165	164605.408747	56.346305
2744.781815	164350.966068	56.351309
2744.233584	164082.427920	56.356314
2743.599853	163839.461714	56.361319
2743.111735	163596.359633	56.366324
2742.148047	163335.330833	56.371329
2741.629097	163080.705078	56.376333
2740.658498	162856.476251	56.381338
2740.295456	162587.996123	56.386343
2739.726987	162329.492976	56.391348
2738.617924	162087.719984	56.396353
2738.282657	161852.958563	56.401357
2737.830796	161595.052515	56.406362
2737.056659	161321.866599	56.411367
2736.413796	161110.348688	56.416372
2735.450836	160837.666816	56.421377
2735.218984	160558.349209	56.426381
2734.085812	160339.399914	56.431386
2733.985898	160070.630101	56.436391
2733.359930	159816.006484	56.441396
2732.465077	159566.067600	56.446401
2731.658834	159289.609809	56.451405
2731.042630	159074.705530	56.456410
2730.296279	158812.111854	56.461415
2729.639569	158552.747711	56.466420
2728.815752	158304.205026	56.471425
2728.202183	158050.889029	56.476429
2727.381760	157802.857910	56.481434
2726.888722	157558.577713	56.486439
2726.356544	157308.470508	56.491444
2725.455576	157059.122720	56.496449
2724.716984	156807.386571	56.501453
2724.158543	156568.907790	56.506458
2723.447305	156330.226069	56.511463
2722.945238	156069.597678	56.516468
2722.429522	155820.261469	56.521473
2721.692670	155571.559574	56.526477
2721.317066	155317.234617	56.531482
2720.344731	155060.857876	56.536487
2719.906512	154802.466344	56.541492
2719.191911	154567.674549	56.546497
2718.457611	154303.245067	56.551501
2717.559372	154055.507856	56.556506
2716.941828	153800.813243	56.561511
2716.229508	153557.588091	56.566516
2715.482342	153311.434047	56.571521
2715.091959	153059.505490	56.576525
2714.063658	152816.628173	56.581530
2713.620217	152566.821730	56.586535
2713.033266	152317.789827	56.591540
2712.362961	152072.319189	56.596545
2711.541924	151819.781964	56.601549
2711.096223	151567.784594	56.606554
2710.307250	151326.799586	56.611559
2709.756485	151080.580255	56.616564
2709.001204	150826.133795	56.621569
2708.659095	150571.242574	56.626573
2707.813126	150328.977585	56.631578
2707.029588	150074.160204	56.636583
2706.660205	149821.782974	56.641588
2705.950378	149575.524006	56.646593
2705.289517	149314.567285	56.651597
2704.336828	149061.220850	56.656602
2703.803220	148810.351828	56.661607
2702.961815	148559.355610	56.666612
2702.390756	148323.289542	56.671617
2701.877866	148059.205940	56.676621
2701.176157	147804.457162	56.681626
2700.481126	147552.746708	56.686631
2700.095705	147304.051932	56.691636
2698.978149	147060.139064	56.696641
2698.367125	146816.414701	56.701645
2697.672917	146571.002511	56.706650
2697.049638	146323.318966	56.711655
2696.613022	146072.697683	56.716660
2695.643963	145820.485328	56.721665
2695.299122	145564.185880	56.726669
2694.849105	145303.203378	56.731674
2693.653283	145056.497403	56.736679
2693.714972	144808.488603	56.741684
2692.426790	144563.999557	56.746689
2691.643069	144309.647958	56.751693
2691.093601	144064.766258	56.756698
2690.337038	143813.108354	56.761703
2690.121606	143566.754499	56.766708
2688.978443	143314.221616	56.771713
2688.488244	143062.832615	56.776717
2687.895482	142820.343839	56.781722
2686.915991	142573.420160	56.786727
2686.344443	142313.829102	56.791732
2685.916044	142073.378657	56.796737
2685.398609	141822.588677	56.801741
2684.338765	141575.368176	56.806746
2683.805589	141329.031902	56.811751
2683.468832	141084.978984	56.816756
2682.353719	140834.507891	56.821761
2681.716826	140578.182035	56.826765
2681.075255	140326.445812	56.831770
2680.434471	140083.541864	56.836775
2679.847591	139837.226313	56.841780
2679.211434	139589.827948	56.846785
2678.448669	139334.561804	56.851789
2678.003543	139093.223052	56.856794
2677.573040	138840.373279	56.861799
2676.926883	138595.004852	56.866804
2675.917441	138344.169468	56.871809
2675.293015	138089.679807	56.876813
2674.740363	137830.365967	56.881818
2674.051832	137584.123337	56.886823
2673.367086	137329.649800	56.891828
2672.955385	137079.022681	56.896833
2672.218575	136822.694281	56.901837
2671.208295	136579.458411	56.906842
2670.690730	136335.879719	56.911847
2670.175590	136070.477669	56.916852
2669.155706	135834.312817	56.921857
2668.866368	135577.975282	56.926861
2668.019528	135330.658841	56.931866
2667.133416	135065.235846	56.936871
2666.557007	134821.336209	56.941876
2665.927115	134575.224072	56.946881
2665.113774	134322.258105	56.951885
2664.426689	134090.831100	56.956890
2663.815868	133841.508407	56.961895
2663.512137	133580.719562	56.966900
2662.933069	133339.005096	56.971905
2662.191961	133086.800757	56.976909
2661.462621	132830.544756	56.981914
2660.639793	132594.515056	56.986919
2660.117278	132342.879687	56.991924
2659.164262	132088.799780	56.996929
2659.059096	131829.507073	57.001933
2658.423599	131575.063930	57.006938
2657.309498	131335.991673	57.011943
2656.887334	131073.796673	57.016948
2656.061043	130817.409185	57.021953
2655.524749	130565.410837	57.026957
2654.708696	130321.067085	57.031962
2654.241983	130080.073999	57.036967
2653.496059	129817.116512	57.041972
2652.908367	129566.659443	57.046977
2652.431633	129316.453766	57.051981
2651.350573	129065.596771	57.056986
2651.091922	128816.694613	57.061991
2650.575880	128562.221921	57.066996
2649.273642	128312.295841	57.072001
2648.974081	128059.673124	57.077005
2648.023636	127806.241465	57.082010
2647.819615	127553.443164	57.087015
2646.870383	127297.564937	57.092020
2645.876753	127055.145080	57.097025
2645.478901	126793.126469	57.102029
2644.906598	126552.600045	57.107034
2643.802466	126303.651481	57.112039
2643.832690	126045.178844	57.117044
2642.734584	125806.520234	57.122049
2642.439482	125546.554617	57.127053
2641.508956	125311.226349	57.132058
2640.857785	125053.175937	57.137063
2640.488432	124799.959603	57.142068
2639.578240	124554.501243	57.147073
2638.964427	124303.702942	57.152077
2638.384517	124053.485736	57.157082
2637.907325	123790.327897	57.162087
2637.210817	123530.293018	57.167092
2636.419825	123293.893715	57.172097
2635.867257	123032.939333	57.177101
2635.153253	122773.778067	57.182106
2634.452646	122524.991085	57.187111
2633.896706	122266.660465	57.192116
2633.022340	122020.203994	57.197121
2632.513767	121751.446442	57.202125
2631.824522	121509.879204	57.207130
2631.021427	121263.723245	57.212135
2630.366097	120998.945378	57.217140
2629.605289	120746.934349	57.222145
2629.003031	120503.134332	57.227149
2628.294347	120249.132831	57.232154
2627.662219	119998.663940	57.237159
2627.195884	119742.299201	57.242164
2626.006568	119498.182640	57.247169
2625.636131	119248.587273	57.252173
2625.162761	119004.774519	57.257178
2624.171645	118748.858243	57.262183
2623.760670	118495.620202	57.267188
2622.843063	118246.609994	57.272193
2622.470228	117987.530997	57.277197
2621.649589	117736.161731	57.282202
2620.794395	117495.235750	57.287207
2620.438008	117246.914349	57.292212
2619.426198	117002.399765	57.297217
2618.974462	116750.886499	57.302221
2618.378387	116499.074876	57.307226
2617.641938	116245.339389	57.312231
2617.078485	115994.168662	57.317236
2616.347576	115745.819681	57.322241
2615.682539	115501.537495	57.327245
2614.853911	115249.844934	57.332250
2614.125417	114999.738435	57.337255
2613.672100	114749.413096	57.342260
2612.943566	114503.760668	57.347265
2612.493002	114253.027288	57.352269
2611.886745	114008.572548	57.357274
2611.041668	113762.457150	57.362279
2610.649858	113508.434366	57.367284
2609.878198	113258.085504	57.372289
2609.063269	113002.605421	57.377293
2608.770275	112769.054371	57.382298
2607.658702	112500.064314	57.387303
2607.103003	112243.497464	57.392308
2606.255590	111994.099880	57.397313
2605.711071	111749.384641	57.402317
2605.238234	111503.676831	57.407322
2604.448568	111251.269575	57.412327
2604.207191	110995.846210	57.417332
2603.043840	110755.960247	57.422337
2602.452975	110501.416017	57.427341
2601.918101	110256.511021	57.432346
2601.485896	109994.941252	57.437351
2601.006127	109744.131210	57.442356
2599.731515	109487.694339	57.447361
2599.460722	109234.324565	57.452365
2598.735871	108973.871808	57.457370
2597.640487	108730.568469	57.462375
2597.138877	108469.089535	57.467380
2596.706842	108227.945017	57.472385
2595.941899	107978.848133	57.477389
2595.325823	107728.791159	57.482394
2594.463176	107475.730267	57.487399
2594.062647	107215.644776	57.492404
2593.140526	106975.142461	57.497409
2592.830593	106717.928559	57.502413
2591.852047	106469.725008	57.507418
2591.286514	106215.069519	57.512423
2590.770047	105962.394819	57.517428
2590.136277	105707.920512	57.522433
2589.576456	105454.636301	57.527437
2588.676229	105202.918698	57.532442
2588.056664	104961.348240	57.537447
2587.470814	104698.102969	57.542452
2586.608006	104448.519108	57.547457
2585.934453	104198.692187	57.552461
2585.377294	103942.664026	57.557466
2584.816235	103691.923789	57.562471
2584.139360	103438.394230	57.567476
2583.509052	103195.631854	57.572481
2582.830272	102931.241083	57.577485
2582.209960	102680.229223	57.582490
2581.336392	102436.384088	57.587495
2580.655036	102170.289543	57.592500
2579.755638	101928.071418	57.597505
2579.223201	101669.672672	57.602509
2578.480620	101413.175046	57.607514
2577.613878	101170.921571	57.612519
2577.036541	100933.033295	57.617524
2576.644463	100691.546905	57.622529
2576.172644	100435.778360	57.627533
2574.981347	100191.176208	57.632538
2574.267132	99936.783644	57.637543
2574.083042	99681.662895	57.642548
2572.888295	99452.958044	57.647553
2572.426522	99198.260897	57.652557
2572.352888	98952.797077	57.657562
2571.082137	98709.808960	57.662567
2570.662262	98456.692728	57.667572
2569.770014	98203.153115	57.672577
2569.248018	97962.172667	57.677581
2568.461364	97716.904904	57.682586
2568.051251	97467.781092	57.687591
2567.539951	97211.236660	57.692596
2566.604492	96973.801405	57.697601
2565.934077	96714.433862	57.702605
2565.549407	96479.313794	57.707610
2564.854529	96222.625749	57.712615
2564.004080	95968.375184	57.717620
2563.434708	95743.565847	57.722625
2562.978660	95472.141927	57.727629
2562.116534	95221.224715	57.732634
2561.228672	94969.287059	57.737639
2560.949995	94726.203525	57.742644
2560.330185	94479.657213	57.747649
2559.517787	94225.350631	57.752653
2559.167247	93973.586352	57.757658
2557.753917	93724.859595	57.762663
2557.682892	93476.113104	57.767668
2556.602685	93227.992250	57.772673
2556.042317	92973.349333	57.777677
2555.192015	92739.629610	57.782682
2554.402831	92492.739057	57.787687
2554.157270	92228.911309	57.792692
2553.336982	91984.136516	57.797697
2552.774444	91744.694110	57.802701
2552.214735	91491.589942	57.807706
2551.470682	91233.889352	57.812711
2551.016339	90982.492629	57.817716
2550.195752	90759.472840	57.822721
2549.558647	90492.963611	57.827725
2548.909582	90248.333225	57.832730
2548.033750	89998.358755	57.837735
2547.980412	89745.980704	57.842740
2546.826133	89500.189810	57.847745
2546.224118	89255.588487	57.852749
2545.763817	88983.870983	57.857754
2544.845492	88752.049534	57.862759
2544.270715	88491.210046	57.867764
2543.170516	88252.335013	57.872769
2542.798626	87996.135311	57.877773
2542.085561	87747.872697	57.882778
2540.930070	87518.396993	57.887783
2540.693238	87257.049767	57.892788
2540.112671	87015.652786	57.897793
2539.407636	86769.010391	57.902797
2538.966790	86520.395534	57.907802
2538.205997	86285.089213	57.912807
2538.158689	86032.981890	57.917812
2537.130352	85784.120089	57.922817
2536.624974	85520.751162	57.927821
2535.845628	85261.061019	57.932826
2535.273014	85020.167108	57.937831
2534.628898	84765.063473	57.942836
2533.736871	84514.185627	57.947841
2532.881191	84267.646827	57.952845
2532.465953	84013.422380	57.957850
2531.920164	83755.051099	57.962855
2531.072233	83506.174812	57.967860
2530.401446	83252.760640	57.972865
2529.779170	83002.130582	57.977869
2529.291776	82745.340636	57.982874
2528.398970	82502.593179	57.987879
2528.109009	82253.034880	57.992884
2527.252481	82003.480642	57.997889
2526.663426	81737.561136	58.002893
2525.973963	81481.230709	58.007898
2525.464779	81238.107605	58.012903
2524.760533	80979.180989	58.017908
2523.978352	80731.436398	58.022913
2523.221845	80469.184644	58.027917
2522.749071	80213.431236	58.032922
2521.582543	79964.121757	58.037927
2521.387654	79716.226525	58.042932
2520.472666	79462.808509	58.047937
2519.602150	79206.414558	58.052941
2519.263561	78958.690636	58.057946
2518.555366	78702.068134	58.062951
2517.948549	78449.393189	58.067956
2516.866611	78203.285344	58.072961
2516.329782	77955.864769	58.077965
2515.806933	77703.521565	58.082970
2514.911722	77456.474339	58.087975
2514.490177	77199.438748	58.092980
2513.600600	76957.003166	58.097985
2513.008062	76708.998288	58.102989
2512.213032	76450.859188	58.107994
2511.392272	76216.709090	58.112999
2510.764768	75971.069432	58.118004
2510.365912	75731.573934	58.123009
2509.833228	75487.933572	58.128013
2509.315081	75232.275093	58.133018
2508.224458	74987.588807	58.138023
2507.792338	74735.375897	58.143028
2507.077261	74490.560103	58.148033
2506.492966	74242.007713	58.153037
2505.795255	73996.523651	58.158042
2504.781992	73748.450847	58.163047
2504.434796	73493.237224	58.168052
2503.463640	73257.023184	58.173057
2502.604659	73014.009417	58.178061
2502.418216	72771.531826	58.183066
2501.615264	72518.651815	58.188071
2501.214302	72279.913750	58.193076
2500.255844	72044.510276	58.198081
2499.710421	71790.882900	58.203085
2498.916543	71553.666488	58.208090
2498.292133	71319.092849	58.213095
2497.935570	71056.861813	58.218100
2496.761821	70816.420626	58.223105
2496.100493	70577.174313	58.228109
2495.814713	70325.222174	58.233114
2494.975304	70086.409112	58.238119
2494.511943	69841.629773	58.243124
2493.719185	69599.654606	58.248129
2492.999624	69347.416427	58.253133
2492.576634	69112.115151	58.258138
2491.865421	68875.367664	58.263143
2491.168791	68617.783356	58.268148
2490.688693	68377.768831	58.273153
2489.737339	68128.002553	58.278157
2489.383354	67871.925478	58.283162
2488.553073	67629.366388	58.288167
2487.736649	67388.945574	58.293172
2486.814261	67145.960653	58.298177
2486.176581	66905.989317	58.303181
2485.841053	66650.720252	58.308186
2485.097092	66412.418455	58.313191
2484.600136	66165.496407	58.318196
2483.627651	65927.835279	58.323201
2482.965599	65679.200996	58.328205
2482.560876	65431.295370	58.333210
2481.877132	65188.040854	58.338215
2481.048026	64956.296179	58.343220
2480.342093	64711.677114	58.348225
2479.846138	64464.529843	58.353229
2479.140292	64219.793586	58.358234
2478.271169	63973.718639	58.363239
2477.881589	63729.153832	58.368244
2476.877680	63492.332117	58.373249
2476.236937	63259.603098	58.378253
2475.767995	63007.183427	58.383258
2475.155658	62770.799346	58.388263
2474.341708	62526.174856	58.393268
2473.741111	62298.890067	58.398273
2473.271264	62045.986339	58.403277
2472.682065	61804.567731	58.408282
2471.819966	61560.435071	58.413287
2471.428533	61307.475005	58.418292
2470.820930	61073.960439	58.423297
2469.417158	60833.804027	58.428301
2469.378581	60584.906550	58.433306
2468.742805	60347.230278	58.438311
2467.985582	60096.101336	58.443316
2466.915237	59858.854689	58.448321
2466.382927	59610.662519	58.453325
2465.670716	59370.722294	58.458330
2464.918922	59140.771302	58.463335
2464.337231	58897.429722	58.468340
2464.055435	58656.499911	58.473345
2463.049574	58413.469302	58.478349
2462.730602	58171.383770	58.483354
2461.812170	57931.504325	58.488359
2461.385514	57690.742960	58.493364
2460.132262	57452.666701	58.498369
2459.913281	57203.441113	58.503373
2459.586988	56974.342048	58.508378
2458.664111	56736.241651	58.513383
2458.129609	56480.198789	58.518388
2457.183550	56240.377376	58.523393
2456.436413	56003.470694	58.528397
2455.955055	55764.401474	58.533402
2455.277773	55523.518324	58.538407
2454.666303	55278.526673	58.543412
2453.671555	55039.418578	58.548417
2452.864344	54801.100312	58.553421
2452.490362	54561.824110	58.558426
2451.509633	54339.620937	58.563431
2451.171984	54092.165245	58.568436
2450.482628	53850.258721	58.573441
2449.985590	53613.751612	58.578445
2449.311040	53381.914457	58.583450
2448.624463	53140.190997	58.588455
2448.008489	52895.216348	58.593460
2446.755911	52669.482308	58.598465
2446.304936	52431.942360	58.603469
2445.981115	52184.187816	58.608474
2445.125754	51955.191450	58.613479
2444.600268	51710.601385	58.618484
2443.635357	51478.916981	58.623489
2443.163693	51249.631478	58.628493
2442.502958	51003.806952	58.633498
2442.151099	50769.193434	58.638503
2441.515838	50532.891050	58.643508
2440.857186	50287.677133	58.648513
2439.726378	50050.630819	58.653517
2439.336278	49804.628018	58.658522
2438.373409	49574.299831	58.663527
2437.770631	49343.170948	58.668532
2437.539324	49097.737983	58.673537
2436.328686	48874.246919	58.678541
2435.683032	48626.260538	58.683546
2434.932172	48399.618276	58.688551
2434.307266	48159.568762	58.693556
2433.429395	47925.471550	58.698561
2432.712452	47703.065256	58.703565
2432.604774	47473.375296	58.708570
2431.076598	47235.689449	58.713575
2430.517089	47014.661813	58.718580
2430.332138	46777.117120	58.723585
2429.616020	46556.619832	58.728589
2428.838961	46319.766685	58.733594
2428.125797	46107.928409	58.738599
2427.719665	45866.932918	58.743604
2426.813100	45651.411294	58.748609
2426.381244	45417.542446	58.753613
2425.638165	45177.343651	58.758618
2425.016140	44965.504765	58.763623
2424.322049	44724.811053	58.768628
2423.585744	44506.230933	58.773633
2422.716145	44277.231842	58.778637
2422.404662	44055.281968	58.783642
2421.555947	43824.641011	58.788647
2420.948347	43589.736682	58.793652
2420.275187	43366.094648	58.798657
2419.502028	43142.183583	58.803661
2419.191370	42910.258298	58.808666
2418.151607	42681.787952	58.813671
2417.707060	42452.846783	58.818676
2417.189586	42230.089687	58.823681
2416.256139	41989.228457	58.828685
2415.632733	41780.198808	58.833690
2414.422413	41555.979238	58.838695
2413.844795	41332.557132	58.843700
2413.479597	41111.469431	58.848705
2412.537483	40888.787573	58.853709
2411.938322	40679.285296	58.858714
2411.006785	40456.839784	58.863719
2410.413398	40244.224308	58.868724
2409.834430	40029.754794	58.873729
2409.158483	39809.202733	58.878733
2408.300607	39593.233674	58.883738
2407.611599	39392.487799	58.888743
2406.896546	39168.126188	58.893748
2406.107358	38956.164874	58.898753
2405.128435	38746.884104	58.903757
2404.756694	38544.509258	58.908762
2403.917242	38352.520613	58.913767
2403.359084	38138.432079	58.918772
2402.259666	37939.377662	58.923777
2401.628255	37737.613211	58.928781
2401.043363	37534.071863	58.933786
2400.110805	37350.791984	58.938791
2399.238550	37157.345799	58.943796
2398.269613	36975.496763	58.948801
2397.090281	36787.681521	58.953805
2396.405439	36614.459349	58.958810
2395.267628	36451.197240	58.963815
2394.537482	36283.557169	58.968820
2393.393721	36123.092034	58.973825
2392.651351	35967.745737	58.978829
2391.751521	35814.294010	58.983834
2390.602434	35685.045813	58.988839
2390.115851	35523.742542	58.993844
2389.224769	35384.544568	58.998849
2388.189797	35254.165800	59.003853
2387.832435	35118.784389	59.008858
2387.111059	34994.757129	59.013863
2386.045994	34865.664739	59.018868
2384.996124	34736.043085	59.023873
2384.316287	34619.670679	59.028877
2384.313730	34490.641863	59.033882
2383.392249	34375.712862	59.038887
2382.840166	34247.509527	59.043892
2382.015673	34129.896038	59.048897
2380.977212	34011.767357	59.053901
2380.670226	33888.769902	59.058906
2380.291343	33774.169903	59.063911
2379.541062	33665.285499	59.068916
2378.816702	33557.099350	59.073921
2378.102614	33432.105975	59.078925
2377.763995	33307.093508	59.083930
2376.683661	33193.142896	59.088935
2376.009985	33080.623495	59.093940
2375.273226	32966.902822	59.098945
2374.473189	32859.771451	59.103949
2374.383241	32735.156853	59.108954
2373.355038	32634.679487	59.113959
2372.503761	32518.410650	59.118964
2371.877894	32409.043893	59.123969
2371.243725	32304.767336	59.128973
2370.986403	32200.850421	59.133978
2369.952497	32088.451799	59.138983
2369.554653	31976.412897	59.143988
2369.056190	31865.100192	59.148993
2368.542090	31761.873042	59.153997
2367.737528	31642.310009	59.159002
2367.109441	31533.848502	59.164007
2366.555338	31431.302894	59.169012
2365.682874	31312.868572	59.174017
2365.120840	31206.116300	59.179021
2364.636971	31099.568794	59.184026
2363.597660	30989.199448	59.189031
2363.118309	30870.821321	59.194036
2362.541708	30758.062240	59.199041
2361.680783	30657.777424	59.204045
2360.899985	30549.106487	59.209050
2360.526078	30444.553990	59.214055
2360.061519	30331.257104	59.219060
2359.536342	30220.523852	59.224065
2358.751861	30101.221679	59.229069
2358.444362	29988.466307	59.234074
2357.407926	29875.693020	59.239079
2356.805779	29780.456800	59.244084
2356.457243	29660.586295	59.249089
2355.468732	29544.527788	59.254093
2354.768776	29421.439624	59.259098
2354.040993	29322.415298	59.264103
2353.587497	29207.378688	59.269108
2353.192945	29096.686069	59.274113
2352.069699	28990.023066	59.279117
2351.682471	28871.363617	59.284122
2351.122863	28760.415092	59.289127
2350.194548	28652.481646	59.294132
2349.537315	28540.251496	59.299137
2348.817316	28429.480753	59.304141
2348.345000	28321.766294	59.309146
2347.493616	28211.548687	59.314151
2346.910148	28098.076093	59.319156
2346.336029	27991.045059	59.324161
2345.728058	27882.244468	59.329165
2345.592962	27758.670177	59.334170
2344.789216	27645.600610	59.339175
2344.200988	27539.360715	59.344180
2343.307557	27426.099175	59.349185
2342.490476	27307.035967	59.354189
2342.019346	27187.577560	59.359194
2341.235284	27076.555331	59.364199
2340.522456	26959.991403	59.369204
2340.092122	26846.153422	59.374209
2339.159608	26730.352633	59.379213
2339.066473	26618.128509	59.384218
2338.101298	26507.503820	59.389223
2337.178166	26386.250412	59.394228
2336.740652	26271.450130	59.399233
2335.748682	26161.501819	59.404237
2335.440381	26041.949479	59.409242
2334.834532	25930.644688	59.414247
2334.418965	25806.950561	59.419252
2333.571405	25692.962622	59.424257
2332.860198	25599.606114	59.429261
2332.085138	25469.420537	59.434266
2331.364643	25362.684493	59.439271
2330.597180	25239.105052	59.444276
2330.225609	25133.044133	59.449281
2329.274604	25012.292018	59.454285
2328.641268	24899.613562	59.459290
2327.941332	24787.352379	59.464295
2327.517720	24667.771722	59.469300
2326.852373	24556.794701	59.474305
2326.202947	24459.151670	59.479309
2325.747768	24339.973328	59.484314
2324.956760	24214.671370	59.489319
2324.113899	24114.264040	59.494324
2323.481004	24002.208599	59.499329
2322.703410	23877.828725	59.504333
2322.326105	23774.253381	59.509338
2321.106572	23672.848841	59.514343
2320.846298	23544.258784	59.519348
2320.272970	23439.346652	59.524353
2318.942489	23328.189151	59.529357
2318.682529	23212.240857	59.534362
2317.927121	23111.092419	59.539367
2317.541444	23007.743709	59.544372
2316.908276	22887.417665	59.549377
2316.260590	22780.978751	59.554381
2315.520337	22658.764491	59.559386
2314.567261	22560.675937	59.564391
2314.093723	22433.185998	59.569396
2313.600242	22337.164185	59.574401
2312.626765	22227.568576	59.579405
2312.279023	22110.459455	59.584410
2311.534503	22002.862281	59.589415
2310.583399	21892.471130	59.594420
2309.896571	21779.235855	59.599425
2309.436288	21674.756493	59.604429
2308.877260	21553.880092	59.609434
2307.793350	21465.000113	59.614439
2307.200598	21356.538454	59.619444
2306.701472	21245.397187	59.624449
2306.185608	21150.260175	59.629453
2305.786124	21031.695964	59.634458
2304.772763	20938.316113	59.639463
2304.140622	20820.907578	59.644468
2303.413556	20712.528509	59.649473
2302.594244	20608.496482	59.654477
2302.253208	20486.270090	59.659482
2301.203118	20394.912938	59.664487
2300.366939	20293.369847	59.669492
2300.010039	20176.468413	59.674497
2299.154909	20078.688488	59.679501
2298.764525	19977.577664	59.684506
2298.176635	19868.059321	59.689511
2297.322567	19772.434831	59.694516
2296.595467	19671.034792	59.699521
2295.786844	19563.982776	59.704525
2295.256404	19452.935753	59.709530
2294.501178	19360.470927	59.714535
2293.742458	19260.203536	59.719540
2293.348746	19157.924634	59.724545
2292.873034	19055.706381	59.729549
2292.262562	18959.231564	59.734554
2291.485077	18854.343700	59.739559
2290.703917	18738.181852	59.744564
2289.861263	18633.454618	59.749569
2289.036671	18535.690568	59.754573
2288.526061	18435.206383	59.759578
2287.718952	18345.286245	59.764583
2286.933593	18248.628856	59.769588
2286.247201	18146.797714	59.774593
2285.528249	18064.353757	59.779597
2284.626326	17968.361529	59.784602
2284.246166	17874.924830	59.789607
2283.337749	17781.298968	59.794612
2282.952676	17688.450476	59.799617
2282.199437	17592.466591	59.804621
2281.800438	17498.883785	59.809626
2280.913810	17414.702709	59.814631
2280.363195	17322.471325	59.819636
2279.868719	17230.670262	59.824641
2279.101237	17150.057315	59.829645
2278.226623	17058.309088	59.834650
2277.355755	16960.895010	59.839655
2277.018863	16867.453181	59.844660
2276.094813	16777.627190	59.849665
2275.317931	16683.213971	59.854669
2274.821855	16598.235608	59.859674
2273.867750	16515.288831	59.864679
2273.208952	16424.795914	59.869684
2272.945414	16339.404014	59.874689
2271.991938	16256.772865	59.879693
2271.079680	16174.718117	59.884698
2270.438417	16087.629191	59.889703
2270.214638	16006.893646	59.894708
2269.667513	15916.938197	59.899713
2268.754467	15842.342912	59.904718
2268.136420	15745.676011	59.909722
2267.394790	15661.566152	59.914727
2266.594184	15579.472204	59.919732
2266.247883	15487.233390	59.924737
2265.486602	15402.968338	59.929742
2264.561916	15327.337566	59.934746
2264.099572	15243.726423	59.939751
2263.325809	15155.931081	59.944756
2262.793057	15072.943695	59.949761
2261.569990	15010.219201	59.954766
2261.660325	14914.635119	59.959770
2260.647794	14839.881755	59.964775
2259.966216	14760.928411	59.969780
2259.288126	14661.724450	59.974785
2258.801615	14583.567084	59.979790
2258.283926	14502.117774	59.984794
2257.455143	14421.630854	59.989799
2256.767434	14341.389124	59.994804
2256.314907	14255.426859	59.999809
2255.209988	14179.727951	60.004814
2254.977912	14083.539350	60.009818
2254.165416	14010.848307	60.014823
2253.252724	13932.766607	60.019828
2252.707930	13850.624676	60.024833
2251.779558	13766.373043	60.029838
2251.359172	13697.244669	60.034842
2250.896373	13623.133198	60.039847
2249.911355	13534.896624	60.044852
2249.386517	13462.467398	60.049857
2248.572210	13388.830879	60.054862
2248.479778	13292.559904	60.059866
2247.590556	13225.143635	60.064871
2246.803618	13136.880312	60.069876
2245.986599	13068.003848	60.074881
2245.450292	12983.033558	60.079886
2244.947743	12914.913399	60.084890
2243.921420	12835.682423	60.089895
2243.493777	12755.758347	60.094900
2242.706373	12688.825841	60.099905
2241.667184	12612.274927	60.104910
2241.359879	12524.070462	60.109914
2240.683321	12465.120075	60.114919
2240.070863	12389.520525	60.119924
2239.310718	12310.013538	60.124929
2238.541975	12243.542049	60.129934
2237.987353	12157.053784	60.134938
2237.145331	12101.194670	60.139943
2236.524865	12017.170498	60.144948
2236.049105	11943.447237	60.149953
2235.268396	11885.154777	60.154958
2234.634774	11793.633852	60.159962
2234.007707	11730.859017	60.164967
2233.002915	11662.802852	60.169972
2232.871214	11588.632209	60.174977
2232.055067	11526.678058	60.179982
2231.226212	11428.473936	60.184986
2230.698581	11380.355470	60.189991
2229.849958	11300.264208	60.194996
2229.507513	11227.303644	60.200001
2228.610217	11164.836383	60.205006
2228.043744	11086.392187	60.210010
2227.520941	11017.882157	60.215015
2226.540057	10945.487000	60.220020
2225.992488	10877.711772	60.225025
2225.197937	10812.417230	60.230030
2224.847503	10737.859395	60.235034
2224.084202	10683.856674	60.240039
2223.269923	10599.822212	60.245044
2222.540630	10532.351544	60.250049
2221.694559	10470.307463	60.255054
2221.173761	10394.431938	60.260058
2220.685304	10334.424478	60.265063
2219.889309	10264.507901	60.270068
2219.352051	10189.261684	60.275073
2218.632666	10126.148007	60.280078
2218.114914	10056.904643	60.285082
2217.057375	9981.640228	60.290087
2216.700704	9924.052592	60.295092
2216.050259	9845.693074	60.300097
2215.107124	9796.690157	60.305102
2214.516466	9720.683946	60.310106
2213.993841	9664.462488	60.315111
2213.000242	9597.146432	60.320116
2212.676054	9525.284697	60.325121
2212.010080	9451.152918	60.330126
2211.355460	9393.499401	60.335130
2210.681679	9328.712058	60.340135
2209.893716	9271.666343	60.345140
2209.731902	9198.265667	60.350145
2208.297915	9138.442581	60.355150
2207.720087	9063.002143	60.360154
2207.015133	9003.067882	60.365159
2206.318882	8929.329270	60.370164
2205.880454	8885.905768	60.375169
2205.381281	8812.915512	60.380174
2204.843475	8746.700524	60.385178
2204.032867	8699.698586	60.390183
2203.268547	8631.836531	60.395188
2203.197342	8558.361503	60.400193
2202.506128	8501.969202	60.405198
2201.596338	8418.805438	60.410202
2201.270048	8361.402009	60.415207
2200.493873	8290.947961	60.420212
2199.833845	8219.753209	60.425217
2198.943254	8143.698854	60.430222
2198.595961	8078.842648	60.435226
2197.284820	8013.914027	60.440231
2196.700761	7951.733110	60.445236
2196.383494	7875.066151	60.450241
2195.507318	7825.222502	60.455246
2194.805372	7757.092238	60.460250
2194.309045	7683.598241	60.465255
2193.333935	7622.170984	60.470260
2192.891010	7559.439211	60.475265
2192.195941	7494.005710	60.480270
2191.956871	7419.225841	60.485274
2190.846810	7366.499002	60.490279
2189.704740	7313.647274	60.495284
2189.299137	7231.176890	60.500289
2188.316723	7174.013077	60.505294
2187.875595	7104.221427	60.510298
2187.371814	7057.652442	60.515303
2186.974356	7002.135817	60.520308
2186.333733	6937.189137	60.525313
2185.337419	6876.178511	60.530318
2184.722795	6804.274984	60.535322
2184.241178	6754.073377	60.540327
2183.318498	6703.108952	60.545332
2182.803410	6636.910783	60.550337
2182.032139	6577.280775	60.555342
2181.314732	6519.593915	60.560346
2180.694445	6451.935869	60.565351
2180.015393	6400.992990	60.570356
2179.548857	6333.579275	60.575361
2178.511321	6285.849559	60.580366
2178.315379	6210.612231	60.585370
2177.727763	6146.472249	60.590375
2176.835982	6096.770191	60.595380
2176.524093	6029.494231	60.600385
2175.212238	5970.347608	60.605390
2174.906885	5905.644096	60.610394
2174.144092	5838.226795	60.615399
2173.525486	5785.532523	60.620404
2173.007879	5726.331059	60.625409
2172.523342	5663.163536	60.630414
2171.841344	5604.904368	60.635418
2171.257876	5542.006244	60.640423
2170.128279	5482.361789	60.645428
2170.028628	5407.140872	60.650433
2169.371381	5353.795686	60.655438
2168.662584	5283.172505	60.660442
2167.622143	5222.518015	60.665447
2166.718320	5159.994146	60.670452
2166.286871	5092.488244	60.675457
2165.450427	5043.848869	60.680462
2164.953580	4973.815831	60.685466
2164.415575	4918.142404	60.690471
2163.610923	4856.887301	60.695476
2163.249618	4792.219628	60.700481
2162.854930	4738.233239	60.705486
2162.188425	4667.176465	60.710490
2161.333091	4611.664174	60.715495
2160.693878	4531.684508	60.720500
2159.942133	4475.710692	60.725505
2158.691174	4430.528848	60.730510
2158.058771	4355.836327	60.735514
2157.732244	4300.216860	60.740519
2157.104440	4241.007302	60.745524
2156.507207	4179.120363	60.750529
2155.916345	4119.429084	60.755534
2155.120802	4051.933674	60.760538
2154.457007	3998.650437	60.765543
2153.739020	3930.233179	60.770548
2153.271409	3868.340391	60.775553
2152.443921	3823.089287	60.780558
2151.717939	3764.310479	60.785562
2151.471442	3692.186265	60.790567
2150.521382	3627.578491	60.795572
2149.728639	3567.735374	60.800577
2148.993749	3518.735580	60.805582
2148.217766	3452.837581	60.810586
2147.498025	3388.377278	60.815591
2146.751705	3344.871027	60.820596
2146.394639	3276.972874	60.825601
2145.715707	3227.370565	60.830606
2145.382306	3168.501890	60.835610
2144.773017	3108.758506	60.840615
2143.817789	3053.301883	60.845620
2143.095586	2989.494324	60.850625
2142.314044	2939.552829	60.855630
2141.566788	2878.185697	60.860634
2140.762152	2835.200436	60.865639
2140.185277	2780.606674	60.870644
2139.892803	2716.474252	60.875649
2138.712095	2667.362740	60.880654
2138.249663	2618.900762	60.885658
2137.545018	2556.585084	60.890663
2137.133480	2489.608455	60.895668
2136.320239	2443.495885	60.900673
2135.881198	2408.846588	60.905678
2135.219571	2351.805980	60.910682
2134.638732	2290.791845	60.915687
2133.460225	2227.819406	60.920692
2133.214375	2164.124391	60.925697
2132.328753	2123.627769	60.930702
2131.639392	2066.874978	60.935706
2130.970792	2012.953139	60.940711
2130.197835	1953.854732	60.945716
2129.945217	1915.384150	60.950721
2129.304917	1859.733066	60.955726
2128.662384	1798.744188	60.960730
2127.653967	1742.407593	60.965735
2126.966417	1682.325270	60.970740
2126.558739	1637.601787	60.975745
2125.542890	1576.345056	60.980750
2125.173924	1514.730454	60.985754
2124.356255	1468.583831	60.990759
2123.855691	1419.390693	60.995764
2123.316541	1363.223967	61.000769
2122.501826	1313.864985	61.005774
2122.065133	1250.177443	61.010778
2121.136025	1207.748199	61.015783
2120.333306	1147.090260	61.020788
2119.655194	1095.827415	61.025793
2119.114500	1041.403173	61.030798
2118.126224	998.910602	61.035802
2117.612462	949.184980	61.040807
2116.928379	908.238722	61.045812
2116.487323	851.813979	61.050817
2115.259120	812.036134	61.055822
2114.919207	765.032193	61.060826
2113.961097	708.040356	61.065831
2113.440310	660.882530	61.070836
2112.639010	626.812208	61.075841
2111.937560	583.551529	61.080846
2111.056477	533.899816	61.085850
2110.496327	497.791989	61.090855
2109.712867	457.283817	61.095860
2109.110361	403.723318	61.100865
2108.623449	383.168290	61.105870
2108.154730	330.063060	61.110874
2107.391473	290.124568	61.115879
2106.278643	247.661859	61.120884
2105.860271	206.776345	61.125889
2104.963483	179.111800	61.130894
2104.181570	148.773604	61.135898
2103.675581	109.788223	61.140903
2102.602893	81.951515	61.145908
2102.085242	65.008139	61.150913
2101.066661	23.131927	61.155918
2100.480216	-6.096882	61.160922
2098.753839	0.646983	61.165927
2093.562277	106.981097	61.170932
2094.013310	101.658523	61.175937
2094.601326	106.254859	61.180942
2095.533895	97.273198	61.185946
2096.122255	98.865524	61.190951
2095.133549	93.419788	61.195956
2094.935037	92.093610	61.200961
2093.199348	93.731490	61.205966
2092.189773	97.502769	61.210970
2091.425085	104.731128	61.215975
2090.402227	110.578116	61.220980
2090.208507	103.870862	61.225985
2089.649375	108.721783	61.230990
2089.092086	109.537177	61.235994
2088.770816	102.930586	61.240999
2088.436211	104.067015	61.246004
2087.883522	107.890365	61.251009
2086.770490	109.585548	61.256014
2085.832724	106.187978	61.261018
2085.317541	103.045030	61.266023
2084.172132	117.688384	61.271028
2083.602795	110.622865	61.276033
2083.679914	114.139696	61.281038
2083.218588	115.390850	61.286042
2082.538232	117.036292	61.291047
2081.750455	110.103207	61.296052
2081.078941	103.970074	61.301057
2080.383245	115.788827	61.306062
2079.221793	116.170272	61.311066
2078.494714	118.233119	61.316071
2077.396433	117.004006	61.321076
2077.617753	110.748100	61.326081
2077.004315	117.583475	61.331086
2076.652434	112.539699	61.336090
2076.041154	104.895819	61.341095
2074.973681	114.958586	61.346100
2074.654366	107.307791	61.351105
2073.629911	117.002627	61.356110
2073.065066	109.425490	61.361114
2072.333919	120.813078	61.366119
2071.670126	111.770952	61.371124
2070.939557	115.441195	61.376129
2070.365808	113.272594	61.381134
2069.398119	114.257198	61.386138
2068.954789	114.477371	61.391143
2068.064506	114.695942	61.396148
2068.455916	104.893449	61.401153
2067.200337	114.716424	61.406158
2065.946064	105.756978	61.411162
2066.074532	101.855901	61.416167
2065.430426	122.836028	61.421172
2064.981998	112.110306	61.426177
2063.342916	114.948650	61.431182
2062.900102	113.793703	61.436186
2062.980008	96.872157	61.441191
2062.021163	117.550584	61.446196
2061.646246	115.071320	61.451201
2060.675005	111.559229	61.456206
2059.453245	115.099283	61.461210
2059.475542	114.442927	61.466215
2058.656072	116.477867	61.471220
2058.369638	110.146435	61.476225
2057.475298	111.005867	61.481230
2056.275695	115.900099	61.486234
2056.115919	116.390648	61.491239
2055.439116	112.226307	61.496244
2054.648884	113.602202	61.501249
2054.190524	121.713896	61.506254
2053.046750	118.681754	61.511258
2052.346511	109.557115	61.516263
2052.168734	115.525448	61.521268
2051.649399	118.859411	61.526273
2051.017389	115.380211	61.531278
2050.328467	113.417542	61.536282
2049.197187	118.288320	61.541287
2048.380922	123.031835	61.546292
2048.348845	110.697850	61.551297
2047.781195	113.752489	61.556302
2046.698454	109.892264	61.561306
2045.952282	110.611494	61.566311
2045.253371	115.724295	61.571316
2045.192822	113.516823	61.576321
2043.959952	117.895971	61.581326
2043.160435	114.126407	61.586330
2043.394850	112.867131	61.591335
2042.052079	121.210654	61.596340
2041.332448	102.932159	61.601345
2040.596362	110.212759	61.606350
2040.698980	105.579382	61.611354
2039.920835	107.451656	61.616359
2038.613545	116.898092	61.621364
2038.017451	108.296223	61.626369
2037.160938	118.059027	61.631374
2037.046786	112.364121	61.636378
2036.414841	104.526423	61.641383
2035.406065	121.398315	61.646388
2035.180466	118.884317	61.651393
2034.458233	108.960544	61.656398
2034.098757	113.716711	61.661402
2033.543789	110.099139	61.666407
2032.438578	115.535038	61.671412
2032.393493	104.854118	61.676417
2031.296886	105.365634	61.681422
2029.828176	114.733619	61.686426
2029.459014	111.137017	61.691431
2028.861466	111.025300	61.696436
2028.684648	111.846546	61.701441
2027.533875	110.389254	61.706446
2027.015028	113.117621	61.711450
2026.624799	105.952733	61.716455
2025.515351	113.529130	61.721460
2025.336113	98.094719	61.726465
2024.974257	115.833706	61.731470
2024.282768	109.855141	61.736474
2023.612494	108.484004	61.741479
2022.177020	108.718164	61.746484
2021.479555	106.832550	61.751489
2021.420302	114.511906	61.756494
2020.325285	107.758492	61.761498
2019.515796	113.694634	61.766503
2019.179736	114.167436	61.771508
2018.525711	109.387662	61.776513
2017.655406	100.988592	61.781518
2016.752398	107.895164	61.786522
2017.062054	106.537216	61.791527
2015.972610	113.810835	61.796532
2015.547355	107.449409	61.801537
2014.937944	106.093845	61.806542
2014.044022	121.056832	61.811546
2013.607458	107.549207	61.816551
2012.501121	124.266288	61.821556
2011.623082	111.450024	61.826561
2011.654450	111.985926	61.831566
2010.740612	112.939927	61.836570
2009.756234	108.064365	61.841575
2009.069058	112.478329	61.846580
2008.626939	109.902514	61.851585
2007.990563	113.952041	61.856590
2007.411525	112.085478	61.861594
2006.931913	105.297465	61.866599
2006.278312	119.265142	61.871604
2005.880425	112.580842	61.876609
2004.489639	111.387151	61.881614
2003.755621	117.689770	61.886618
2003.340097	112.206699	61.891623
2002.467117	111.116890	61.896628
2002.005613	107.430877	61.901633
2001.241237	115.537533	61.906638
2000.608587	125.200164	61.911642
2000.598633	109.256351	61.916647
1999.912369	123.563515	61.921652
1999.550137	109.586798	61.926657
1998.426914	120.918366	61.931662
1997.596785	115.971016	61.936666
1996.780940	116.788048	61.941671
1995.827331	118.368080	61.946676
1995.557037	118.910867	61.951681
1995.069737	116.982438	61.956686
1994.485270	110.345105	61.961690
1993.608787	108.418532	61.966695
1992.722552	123.142197	61.971700
1991.787703	115.642735	61.976705
1991.260628	113.600778	61.981710
1990.723537	113.660814	61.986714
1990.412662	108.457590	61.991719
1989.651895	124.265155	61.996724
1989.090321	113.486455	62.001729
1988.783167	116.346798	62.006734
1988.106121	122.377039	62.011738
1986.931172	108.234457	62.016743
1985.933199	123.586113	62.021748
1985.151947	112.561601	62.026753
1984.717964	117.074146	62.031758
1984.277885	120.239428	62.036762
1983.766270	112.250185	62.041767
1983.237619	121.979882	62.046772
1982.463408	110.273044	62.051777
1982.572037	110.790374	62.056782
1981.023265	113.964497	62.061786
1980.430961	102.477937	62.066791
1979.562847	119.133552	62.071796
1979.168914	109.685940	62.076801
1978.730918	113.456412	62.081806
1977.663053	118.985747	62.086810
1976.643111	104.837492	62.091815
1976.370970	116.950129	62.096820
1975.661140	109.236771	62.101825
1974.513169	112.276315	62.106830
1973.754983	112.472371	62.111834
1974.384249	109.846334	62.116839
1973.128433	113.809703	62.121844
1972.416588	109.173156	62.126849
1971.915789	118.480559	62.131854
1970.922425	119.535502	62.136858
1970.865567	108.049095	62.141863
1969.882685	110.042194	62.146868
1968.960026	102.979186	62.151873
1968.120270	110.389793	62.156878
1967.708363	112.659667	62.161882
1967.254113	115.587515	62.166887
1966.790602	107.645834	62.171892
1966.288032	113.440231	62.176897
1965.589707	103.935296	62.181902
1964.363762	125.010944	62.186906
1963.698433	100.389544	62.191911
1962.747443	123.239682	62.196916
1962.476521	116.735499	62.201921
1961.825152	118.910931	62.206926
1961.108363	110.023907	62.211930
1961.447006	106.896826	62.216935
1960.575751	115.409944	62.221940
1959.173387	116.245981	62.226945
1958.498280	113.323980	62.231950
1957.792653	108.095122	62.236954
1957.412586	109.478468	62.241959
1956.747677	110.418200	62.246964
1956.601100	103.528449	62.251969
1955.131686	111.392237	62.256974
1954.098132	126.831548	62.261978
1953.844911	110.341338	62.266983
1953.015697	121.834395	62.271988
1952.711572	119.600942	62.276993
1952.557552	105.944410	62.281998
1951.673610	123.181261	62.287002
1951.069676	117.054782	62.292007
1949.606863	121.850501	62.297012
1949.040258	105.242899	62.302017
1948.590673	113.018906	62.307022
1948.216854	110.575756	62.312026
1947.775088	114.600709	62.317031
1947.058913	109.250531	62.322036
1946.034892	112.822317	62.327041
1945.190434	108.888042	62.332046
1944.512266	108.839603	62.337050
1944.197539	105.891935	62.342055
1943.578383	121.632868	62.347060
1943.446783	107.012459	62.352065
1942.774260	117.096141	62.357070
1941.223017	110.976560	62.362074
1940.855616	113.155798	62.367079
1939.853417	105.517252	62.372084
1939.429479	111.201403	62.377089
1939.238198	106.095891	62.382094
1938.050772	109.608469	62.387098
1937.597991	95.515278	62.392103
1936.490906	109.274260	62.397108
1936.089154	115.591948	62.402113
1935.780823	107.961515	62.407118
1934.894461	112.214737	62.412122
1934.711121	98.198612	62.417127
1933.308109	115.341251	62.422132
1932.503754	108.021366	62.427137
1932.018657	103.706787	62.432142
1931.131060	103.021427	62.437146
1931.312433	107.784773	62.442151
1930.385351	112.782440	62.447156
1930.071263	110.782375	62.452161
1928.733868	100.770238	62.457166
1927.973454	112.181410	62.462170
1927.642820	102.894069	62.467175
1926.858950	98.816151	62.472180
1926.527629	108.623322	62.477185
1926.120528	106.283227	62.482190
1924.716394	105.337691	62.487194
1924.168230	108.242608	62.492199
1923.609009	104.874887	62.497204
1923.070113	115.527108	62.502209
1922.561218	98.774750	62.507214
1921.977192	119.310117	62.512218
1921.336827	98.248526	62.517223
1920.145375	118.667449	62.522228
1919.667431	121.627449	62.527233
1919.249934	102.708139	62.532238
1918.607993	117.038229	62.537242
1918.050165	105.992471	62.542247
1916.801592	114.048287	62.547252
1916.182295	112.757391	62.552257
1915.709633	118.936537	62.557262
1914.585222	116.885358	62.562266
1914.514340	110.505538	62.567271
1914.187434	121.756436	62.572276
1913.460780	110.136690	62.577281
1912.617606	108.286855	62.582286
1911.619332	124.878000	62.587290
1911.261375	102.282998	62.592295
1910.589610	108.958930	62.597300
1909.602317	111.422660	62.602305
1908.853548	104.098691	62.607310
1908.057914	105.557482	62.612314
1907.636489	108.199441	62.617319
1907.280659	117.247300	62.622324
1906.525223	116.310742	62.627329
1906.384356	113.918918	62.632334
1905.491056	111.539329	62.637338
1904.809700	94.205690	62.642343
1903.798594	117.253017	62.647348
1903.336607	113.543447	62.652353
1902.993110	102.055258	62.657358
1901.727429	111.963471	62.662362
1901.288653	116.032107	62.667367
1900.465962	114.992692	62.672372
1900.016144	110.284606	62.677377
1899.630057	107.956948	62.682382
1898.826667	106.312104	62.687386
1897.883873	111.168778	62.692391
1896.842536	109.158033	62.697396
1896.775146	99.991324	62.702401
1896.570514	112.091660	62.707406
1895.192264	109.084206	62.712410
1894.401873	95.248049	62.717415
1893.500667	101.851605	62.722420
1893.015779	110.491041	62.727425
1892.841647	110.610159	62.732430
1892.049624	112.956163	62.737434
1891.847600	108.670762	62.742439
1890.742068	110.658132	62.747444
1889.845795	108.577051	62.752449
1888.950822	100.801665	62.757454
1888.351410	109.388325	62.762458
1888.559702	103.768392	62.767463
1887.845955	111.993180	62.772468
1887.018288	101.811832	62.777473
1886.369687	104.051491	62.782478
1885.264030	111.270958	62.787482
1884.958097	98.933183	62.792487
1883.660348	107.274346	62.797492
1882.970810	108.722607	62.802497
1882.481754	113.775314	62.807502
1881.759296	110.357830	62.812506
1881.563745	98.776776	62.817511
1880.818695	112.175534	62.822516
1880.362765	111.222966	62.827521
1880.119109	111.558117	62.832526
1878.866712	118.446092	62.837530
1878.168039	100.795100	62.842535
1877.543193	119.987144	62.847540
1876.857875	102.020232	62.852545
1875.991537	105.734153	62.857550
1875.115831	119.916871	62.862554
1874.684025	104.216678	62.867559
1874.299734	107.983365	62.872564
1873.875132	108.124907	62.877569
1873.589501	107.992084	62.882574
1871.882726	107.862569	62.887578
1871.657014	101.562532	62.892583
1870.841676	112.662329	62.897588
1870.371131	109.640068	62.902593
1869.880923	105.927104	62.907598
1868.161217	98.085570	62.912602
1867.564514	120.739118	62.917607
1867.150536	114.147286	62.922612
1866.980948	121.115638	62.927617
1866.729647	106.317142	62.932622
1865.810677	110.860976	62.937626
1865.394817	108.370902	62.942631
1863.820630	117.151769	62.947636
1863.239430	108.255868	62.952641
1862.689016	105.597935	62.957646
1861.887730	118.502607	62.962650
1861.776724	110.128107	62.967655
1861.606580	114.838457	62.972660
1860.909090	107.968387	62.977665
1860.206876	106.394218	62.982670
1859.388679	113.837698	62.987674
1858.578218	110.189779	62.992679
1857.362702	105.653745	62.997684
1856.981061	112.939601	63.002689
1856.266308	114.219993	63.007694
1855.729614	116.943338	63.012698
1855.501865	111.901971	63.017703
1854.386113	104.921708	63.022708
1853.581737	108.892289	63.027713
1853.383514	114.483841	63.032718
1852.356949	121.690766	63.037722
1851.950745	115.829374	63.042727
1851.082323	117.954145	63.047732
1850.334116	113.982544	63.052737
1849.507979	110.527919	63.057742
1849.081745	116.986691	63.062746
1848.669121	111.534732	63.067751
1847.839231	112.536956	63.072756
1846.690274	96.244215	63.077761
1846.525999	103.908694	63.082766
1845.819512	115.759152	63.087770
1845.597659	111.139452	63.092775
1844.994201	113.690483	63.097780
1844.008614	106.798360	63.102785
1843.272368	102.799635	63.107790
1842.470238	105.328598	63.112794
1841.858370	103.848893	63.117799
1840.773915	105.593251	63.122804
1840.284507	105.180568	63.127809
1839.819772	101.596025	63.132814
1839.356042	108.308318	63.137818
1838.826779	106.088557	63.142823
1838.080975	106.039847	63.147828
1836.971171	105.184810	63.152833
1836.513418	104.100083	63.157838
1835.905202	111.431380	63.162842
1835.784264	110.673196	63.167847
1834.416076	116.332266	63.172852
1833.296400	111.818868	63.177857
1833.138503	98.025796	63.182862
1832.628088	113.930801	63.187866
1832.592693	104.229188	63.192871
1831.545718	123.308504	63.197876
1830.229290	121.507039	63.202881
1829.973943	113.563874	63.207886
1829.271345	98.499607	63.212890
1828.943924	118.286208	63.217895
1828.167375	119.497577	63.222900
1826.819445	111.988095	63.227905
1826.098598	99.098086	63.232910
1825.573196	132.773723	63.237914
1825.633580	107.940953	63.242919
1825.027698	107.453733	63.247924
1824.450203	115.578054	63.252929
1823.694730	100.441764	63.257934
1822.569126	131.159879	63.262938
1822.556598	110.449605	63.267943
1821.132043	109.661902	63.272948
1820.121916	123.413416	63.277953
1820.164692	93.539040	63.282958
1819.348605	126.743608	63.287962
1819.112794	113.483267	63.292967
1818.519731	97.346683	63.297972
1817.193011	118.165558	63.302977
1816.642230	113.227530	63.307982
1816.096631	111.011945	63.312986
1815.637668	101.290869	63.317991
1815.225191	100.741401	63.322996
1813.734992	118.060348	63.328001
1813.488759	108.791164	63.333006
1812.460147	115.184757	63.338010
1812.125097	105.541768	63.343015
1811.705257	105.592682	63.348020
1810.818230	117.003484	63.353025
1810.139313	106.005376	63.358030
1809.186333	117.240581	63.363034
1808.928998	109.258315	63.368039
1808.191890	102.490746	63.373044
1807.758193	116.713662	63.378049
1807.063327	105.651859	63.383054
1806.079849	104.671124	63.388058
1805.679866	105.754893	63.393063
1805.275630	105.822253	63.398068
1803.908752	109.320807	63.403073
1803.524611	103.200474	63.408078
1802.335523	112.197742	63.413082
1802.245718	117.791001	63.418087
1801.513206	102.870258	63.423092
1801.199816	118.901668	63.428097
1800.779699	108.849587	63.433102
1799.218267	102.499920	63.438106
1798.600094	119.563702	63.443111
1798.501293	101.481608	63.448116
1797.798754	101.492268	63.453121
1797.236026	108.553007	63.458126
1796.232223	103.650663	63.463130
1796.095925	93.884664	63.468135
1795.060427	92.869620	63.473140
1794.100364	113.124091	63.478145
1793.645461	119.746686	63.483150
1792.975055	94.113840	63.488154
1792.584068	121.418031	63.493159
1792.236847	97.335961	63.498164
1790.610591	109.759823	63.503169
1790.168697	81.764819	63.508174
1789.508794	121.077025	63.513178
1789.502947	104.553890	63.518183
1788.849065	98.684546	63.523188
1787.832884	115.114553	63.528193
1787.350252	105.334167	63.533198
1786.170809	103.654468	63.538202
1785.666772	106.418367	63.543207
1784.544055	112.697608	63.548212
1783.962700	112.619644	63.553217
1783.636465	92.834390	63.558222
1782.580001	114.398787	63.563226
1782.791803	101.985119	63.568231
1782.209392	99.788004	63.573236
1781.275272	125.631546	63.578241
1780.940093	108.216161	63.583246
1780.044819	110.031419	63.588250
1779.450322	101.916638	63.593255
1778.264044	113.800725	63.598260
1777.310917	106.930285	63.603265
1776.959912	104.805224	63.608270
1776.577121	113.537262	63.613274
1776.347763	102.426774	63.618279
1775.156787	110.277963	63.623284
1774.068520	119.197736	63.628289
1773.840501	100.467575	63.633294
1772.850851	96.135401	63.638298
1772.838938	116.783319	63.643303
1772.622146	104.049807	63.648308
1771.039375	108.747975	63.653313
1770.846550	93.276366	63.658318
1769.955841	108.166337	63.663322
1769.394168	114.416401	63.668327
1768.611501	113.581975	63.673332
1767.586364	104.013905	63.678337
1767.434338	97.605995	63.683342
1766.907426	119.587744	63.688346
1765.765478	99.900501	63.693351
1765.089521	102.778434	63.698356
1764.135924	97.999013	63.703361
1763.980539	97.307802	63.708366
1763.267492	109.772712	63.713370
1763.127909	114.979657	63.718375
1762.363952	94.552757	63.723380
1761.077115	106.088557	63.728385
1760.949800	110.740069	63.733390
1759.560669	106.334155	63.738394
1759.137185	95.358581	63.743399
1757.956118	99.605044	63.748404
1757.962630	101.660264	63.753409
1757.729836	99.533778	63.758414
1757.022791	105.436364	63.763418
1756.257343	92.914578	63.768423
1755.309128	109.288061	63.773428
1754.407278	108.259690	63.778433
1754.410148	105.264762	63.783438
1753.579916	104.515162	63.788442
1752.639774	101.846618	63.793447
1751.647568	105.965323	63.798452
1751.136073	109.648153	63.803457
1751.040546	103.445723	63.808462
1750.419064	107.809885	63.813466
1749.150169	109.731799	63.818471
1748.659635	107.154265	63.823476
1748.053095	106.921044	63.828481
1747.892972	87.951477	63.833486
1746.643086	100.265115	63.838490
1746.107674	107.892350	63.843495
1745.131090	100.219870	63.848500
1744.603889	107.222936	63.853505
1744.348100	96.460416	63.858510
1743.770806	117.209164	63.863514
1743.004964	103.528433	63.868519
1742.287051	104.255874	63.873524
1741.799052	112.170457	63.878529
1740.912542	99.218490	63.883534
1739.899812	114.668720	63.888538
1739.170952	102.793947	63.893543
1738.847675	109.146492	63.898548
1738.072166	108.911727	63.903553
1737.927746	100.973043	63.908558
1736.747572	113.460116	63.913562
1735.978444	110.411195	63.918567
1735.632072	102.667005	63.923572
1735.013318	109.837572	63.928577
1734.851995	104.517605	63.933582
1733.724240	112.204235	63.938586
1732.854677	102.865350	63.943591
1732.682744	98.087939	63.948596
1731.376577	104.516176	63.953601
1730.543571	98.853488	63.958606
1729.667459	97.603430	63.963610
1729.126440	95.797127	63.968615
1728.864815	104.486264	63.973620
1728.644245	111.879002	63.978625
1728.625467	112.473324	63.983630
1727.127309	107.181197	63.988634
1726.365350	98.321942	63.993639
1725.845263	106.460805	63.998644
1724.843648	108.963143	64.003649
1724.293006	106.849300	64.008654
1723.243196	109.676244	64.013658
1723.077253	97.705764	64.018663
1722.740388	104.814210	64.023668
1721.574023	104.028129	64.028673
1721.142965	97.867961	64.033678
1720.134952	110.113237	64.038682
1719.849623	103.781694	64.043687
1719.453251	93.549264	64.048692
1718.178194	95.908963	64.053697
1717.813771	106.880395	64.058702
1716.948470	106.148992	64.063706
1716.487129	103.013345	64.068711
1715.807234	98.543689	64.073716
1714.404463	99.946016	64.078721
1714.189211	96.206762	64.083726
1713.673122	98.977316	64.088730
1713.589969	98.303020	64.093735
1713.074542	93.859279	64.098740
1711.641657	103.644313	64.103745
1711.422015	102.835585	64.108750
1710.725111	104.288212	64.113754
1709.665670	105.703813	64.118759
1708.809129	102.962085	64.123764
1707.829979	98.330242	64.128769
1707.909698	96.966211	64.133774
1707.319477	97.130934	64.138778
1707.047055	98.624940	64.143783
1706.168113	101.262330	64.148788
1705.251554	98.142227	64.153793
1704.658963	97.564620	64.158798
1703.820567	107.144849	64.163802
1702.863867	96.514172	64.168807
1702.305288	102.208691	64.173812
1701.663255	100.752735	64.178817
1701.502997	93.258101	64.183822
1700.991301	106.840572	64.188826
1699.884586	100.458166	64.193831
1698.917698	94.119781	64.198836
1698.345747	102.077659	64.203841
1698.169439	105.858633	64.208846
1697.502486	109.876809	64.213850
1696.722502	95.641717	64.218855
1695.644122	102.921564	64.223860
1694.700610	109.054105	64.228865
1695.204516	100.003244	64.233870
1694.270139	102.862322	64.238874
1693.347575	109.579709	64.243879
1692.907531	99.147649	64.248884
1692.028679	95.570577	64.253889
1691.452668	98.538301	64.258894
1690.231203	107.069264	64.263898
1689.382504	100.081358	64.268903
1689.154789	104.722009	64.273908
1688.848865	106.080997	64.278913
1688.528288	100.437846	64.283918
1687.745470	107.970354	64.288922
1686.822624	105.239167	64.293927
1686.364851	101.819123	64.298932
1685.445206	103.570476	64.303937
1684.724148	103.293964	64.308942
1683.973658	94.185337	64.313946
1683.751599	92.132846	64.318951
1682.746239	103.869952	64.323956
1681.579634	105.192205	64.328961
1681.192997	94.046807	64.333966
1680.220236	108.606069	64.338970
1680.260201	96.624965	64.343975
1680.169531	115.446739	64.348980
1678.966563	114.739027	64.353985
1678.492955	91.859743	64.358990
1677.652545	102.864209	64.363994
1676.379987	100.768868	64.368999
1675.853267	91.899075	64.374004
1675.098526	102.350643	64.379009
1674.533165	88.666493	64.384014
1674.282394	100.939708	64.389018
1673.934499	93.250968	64.394023
1673.182809	99.096010	64.399028
1672.077248	101.238004	64.404033
1671.753251	94.002761	64.409038
1670.965687	98.305014	64.414042
1669.894879	88.819948	64.419047
1669.419614	94.592693	64.424052
1668.727643	97.585149	64.429057
1668.362375	86.420597	64.434062
1667.775392	101.811080	64.439066
1666.795447	96.334178	64.444071
1666.232422	90.343216	64.449076
1665.559841	104.361231	64.454081
1665.211779	87.640203	64.459086
1664.025875	95.440160	64.464090
1663.414724	93.428981	64.469095
1663.153492	89.279170	64.474100
1662.507082	89.135877	64.479105
1661.798312	95.891840	64.484110
1660.801140	102.912807	64.489114
1660.037776	96.732907	64.494119
1659.784974	97.834313	64.499124
1659.305766	102.177466	64.504129
1658.261320	98.234072	64.509134
1657.186039	105.612784	64.514138
1656.848334	106.776562	64.519143
1656.662526	103.907800	64.524148
1655.804193	107.478595	64.529153
1654.714186	99.926672	64.534158
1653.932990	99.074703	64.539162
1653.599525	92.583675	64.544167
1653.470776	93.338961	64.549172
1652.456219	96.973995	64.554177
1651.727556	92.948901	64.559182
1651.002324	103.608663	64.564186
1650.388436	95.892801	64.569191
1650.193158	94.963521	64.574196
1648.634889	105.618437	64.579201
1648.304476	90.794737	64.584206
1647.488899	89.911964	64.589210
1647.192510	93.111225	64.594215
1646.984447	97.272539	64.599220
1645.741065	99.221984	64.604225
1645.208306	94.088767	64.609230
1644.709103	95.882143	64.614234
1643.529281	102.181541	64.619239
1642.781846	93.750500	64.624244
1642.158903	104.155906	64.629249
1641.849571	94.683912	64.634254
1641.210383	97.412537	64.639258
1640.699583	97.544157	64.644263
1639.998776	96.747227	64.649268
1639.350210	105.622410	64.654273
1639.007135	91.385743	64.659278
1637.831553	95.060554	64.664282
1636.860720	95.971699	64.669287
1636.587147	89.477468	64.674292
1635.829860	99.755989	64.679297
1635.471669	92.286503	64.684302
1634.164698	94.468394	64.689306
1633.767380	94.116810	64.694311
1633.442553	89.518237	64.699316
1633.031429	102.014035	64.704321
1631.962169	98.079325	64.709326
1631.132365	100.264254	64.714330
1630.237741	103.159613	64.719335
1630.542222	93.457648	64.724340
1629.067521	95.828607	64.729345
1628.202626	93.447764	64.734350
1627.692286	101.649739	64.739354
1627.262291	98.047109	64.744359
1626.615026	85.785715	64.749364
1625.936160	86.631555	64.754369
1625.044790	100.175001	64.759374
1624.832145	97.665304	64.764378
1624.203427	101.414081	64.769383
1623.833207	105.385129	64.774388
1622.710920	103.649121	64.779393
1622.253016	93.915322	64.784398
1621.120872	102.164050	64.789402
1620.749708	91.430929	64.794407
1619.891223	84.384691	64.799412
1618.705457	98.764921	64.804417
1618.706690	105.081682	64.809422
1618.162822	99.548133	64.814426
1617.615489	99.888979	64.819431
1616.788427	98.670590	64.824436
1615.813271	102.625789	64.829441
1615.500017	92.354953	64.834446
1614.979905	94.317227	64.839450
1614.204963	99.229315	64.844455
1613.238192	89.265726	64.849460
1612.390868	98.292329	64.854465
1612.217094	91.564638	64.859470
1611.654289	97.374952	64.864474
1610.578426	98.102530	64.869479
1610.097914	94.739731	64.874484
1609.253627	106.023935	64.879489
1609.005759	99.167671	64.884494
1608.019503	110.088101	64.889498
1606.959716	98.300655	64.894503
1606.628383	91.855028	64.899508
1605.914591	102.298524	64.904513
1605.610615	96.012543	64.909518
1605.326790	95.210869	64.914522
1604.424714	103.437242	64.919527
1603.456200	109.258408	64.924532
1602.776366	101.184048	64.929537
1602.242425	90.019503	64.934542
1601.231201	93.513682	64.939546
1600.530848	105.989209	64.944551
1600.442655	94.424273	64.949556
1599.744753	98.226622	64.954561
1599.176676	104.026740	64.959566
1598.361437	106.171521	64.964570
1597.950388	101.941445	64.969575
1596.957019	89.605746	64.974580
1596.052162	101.506667	64.979585
1595.336499	104.310528	64.984590
1594.898431	107.502347	64.989594
1594.375595	98.805413	64.994599
1594.005109	95.226450	64.999604
1592.405535	104.213319	65.004609
1592.212681	91.040839	65.009614
1591.595347	103.220914	65.014618
1591.235737	99.316964	65.019623
1590.421817	92.082315	65.024628
1589.665189	98.011733	65.029633
1589.376224	100.080781	65.034638
1588.455161	106.186132	65.039642
1587.168060	109.971723	65.044647
1586.951063	95.516349	65.049652
1586.175295	96.327136	65.054657
1585.893340	100.823451	65.059662
1584.922159	101.565945	65.064666
1584.033721	106.090820	65.069671
1583.557467	91.447998	65.074676
1582.807289	108.151148	65.079681
1582.820942	96.886982	65.084686
1581.965239	107.091273	65.089690
1581.118100	104.326021	65.094695
1580.931929	94.091767	65.099700
1579.845486	104.999735	65.104705
1578.980776	96.593659	65.109710
1578.115077	103.352500	65.114714
1577.478679	96.084916	65.119719
1577.771883	95.227829	65.124724
1576.194378	99.616199	65.129729
1575.900132	99.174134	65.134734
1575.116441	96.559646	65.139738
1574.472941	98.211968	65.144743
1573.701902	97.549211	65.149748
1572.676443	101.193890	65.154753
1571.835602	97.664437	65.159758
1571.838633	96.907069	65.164762
1571.584287	96.244211	65.169767
1571.141885	93.698491	65.174772
1569.880740	109.303336	65.179777
1569.387657	97.265024	65.184782
1568.527584	99.934150	65.189786
1567.396494	89.861082	65.194791
1566.712566	82.050733	65.199796
1566.044694	97.718985	65.204801
1565.557966	99.040486	65.209806
1565.331588	95.127987	65.214810
1564.753646	110.501280	65.219815
1564.472571	88.277399	65.224820
1563.157765	90.919437	65.229825
1562.919574	94.978313	65.234830
1562.195119	93.978592	65.239834
1561.086823	93.520807	65.244839
1560.369482	88.584092	65.249844
1559.726655	98.010275	65.254849
1559.302011	90.962928	65.259854
1558.649148	98.220934	65.264858
1557.389176	101.045065	65.269863
1557.344330	87.786003	65.274868
1556.610504	91.095778	65.279873
1556.319177	93.121052	65.284878
1555.063143	89.389513	65.289882
1554.404048	96.188064	65.294887
1554.243779	89.593847	65.299892
1553.601360	97.201835	65.304897
1552.727071	94.245378	65.309902
1551.904714	88.962673	65.314906
1551.292834	100.594710	65.319911
1551.118598	90.339645	65.324916
1549.830359	88.920185	65.329921
1548.813558	92.747989	65.334926
1548.476429	96.537173	65.339930
1548.023176	91.924331	65.344935
1548.056501	88.716427	65.349940
1546.538698	104.950230	65.354945
1545.976245	92.003638	65.359950
1545.351910	98.959085	65.364954
1545.025446	94.671429	65.369959
1544.313196	83.388593	65.374964
1543.052121	94.286470	65.379969
1542.689227	90.584892	65.384974
1542.185670	93.321945	65.389978
1541.354834	95.395107	65.394983
1540.933882	95.873573	65.399988
1539.893198	93.779302	65.404993
1539.299054	97.237188	65.409998
1539.188505	90.437963	65.415002
1538.038548	100.004657	65.420007
1537.449913	93.885343	65.425012
1536.516809	108.821513	65.430017
1536.328044	93.920144	65.435022
1535.857047	97.632837	65.440026
1534.683584	90.098972	65.445031
1534.172867	87.592500	65.450036
1533.359723	97.687536	65.455041
1533.022736	87.664908	65.460046
1531.852413	94.029064	65.465050
1530.788122	90.568251	65.470055
1530.842716	89.884687	65.475060
1530.254229	91.034717	65.480065
1530.019323	84.616360	65.485070
1529.473420	94.486011	65.490074
1528.596393	94.666389	65.495079
1527.995084	88.572747	65.500084
1526.374485	91.458929	65.505089
1525.431546	86.654265	65.510094
1525.363941	92.381166	65.515098
1524.908511	94.284296	65.520103
1524.719953	82.818904	65.525108
1523.565966	80.051980	65.530113
1522.848659	89.010630	65.535118
1522.279484	85.155768	65.540122
1521.511431	98.403684	65.545127
1521.151871	90.977016	65.550132
1520.288607	92.104485	65.555137
1519.678316	90.366006	65.560142
1519.329785	91.058459	65.565146
1518.238984	89.434185	65.570151
1517.561878	87.170189	65.575156
1516.762398	87.257828	65.580161
1516.380695	81.129294	65.585166
1516.050281	92.860095	65.590170
1514.892001	87.398988	65.595175
1514.244193	92.275126	65.600180
1513.579216	100.828098	65.605185
1513.104780	91.249916	65.610190
1512.756490	97.808281	65.615194
1511.400440	99.141792	65.620199
1511.296081	84.239640	65.625204
1510.447845	92.476397	65.630209
1509.614950	94.232944	65.635214
1508.946762	94.652939	65.640218
1507.970198	96.916418	65.645223
1507.885945	83.822894	65.650228
1507.226282	99.884065	65.655233
1506.660770	95.539792	65.660238
1505.626982	98.279119	65.665242
1504.770708	98.889846	65.670247
1505.050561	94.450652	65.675252
1503.904238	96.452543	65.680257
1502.827968	82.302483	65.685262
1502.274258	84.924516	65.690266
1501.776321	80.607355	65.695271
1501.566034	89.704618	65.700276
1500.413527	84.367175	65.705281
1499.663946	88.422172	65.710286
1499.356744	84.276537	65.715290
1498.488748	91.538779	65.720295
1497.679296	78.978381	65.725300
1497.023585	95.950350	65.730305
1496.651266	87.475523	65.735310
1495.975335	90.415009	65.740314
1495.272839	90.176599	65.745319
1494.495512	93.501188	65.750324
1493.634927	91.441390	65.755329
1493.257000	91.477810	65.760334
1492.932257	89.733379	65.765338
1491.589059	94.223323	65.770343
1491.016868	91.409679	65.775348
1490.567288	90.823587	65.780353
1490.432381	81.902625	65.785358
1489.372669	91.218458	65.790362
1488.226499	94.425058	65.795367
1487.953483	93.120237	65.800372
1487.375644	101.988930	65.805377
1486.687384	88.933054	65.810382
1485.751747	87.743003	65.815386
1484.839249	90.590786	65.820391
1484.685954	81.619134	65.825396
1484.368539	94.240377	65.830401
1483.603826	89.090454	65.835406
1482.887597	88.040566	65.840410
1481.899432	92.647545	65.845415
1481.617824	93.212678	65.850420
1480.274398	90.767600	65.855425
1479.527097	91.532896	65.860430
1479.220644	86.321183	65.865434
1478.612495	95.879051	65.870439
1478.559009	83.348316	65.875444
1477.299262	94.993441	65.880449
1476.799448	89.314168	65.885454
1476.402434	92.283443	65.890458
1475.129003	86.225680	65.895463
1474.514355	87.666869	65.900468
1473.718950	94.362524	65.905473
1473.206976	90.377164	65.910478
1472.990877	98.417277	65.915482
1472.393765	91.914575	65.920487
1471.504977	83.163891	65.925492
1471.042073	81.148125	65.930497
1470.209697	89.297218	65.935502
1469.189035	100.473867	65.940506
1468.363684	103.580605	65.945511
1467.924111	93.525411	65.950516
1467.482544	88.975381	65.955521
1467.182208	95.007338	65.960526
1466.508616	93.378275	65.965530
1465.659341	93.675683	65.970535
1465.074093	86.614465	65.975540
1464.055634	103.814400	65.980545
1463.035928	90.038545	65.985550
1462.672739	87.721519	65.990554
1461.957200	105.018382	65.995559
1461.897626	98.001337	66.000564
1461.237235	96.881083	66.005569
1460.195552	94.104221	66.010574
1459.760724	91.166257	66.015578
1458.750280	91.938690	66.020583
1458.134199	93.179849	66.025588
1457.200467	98.077791	66.030593
1456.566207	110.124965	66.035598
1456.549600	91.976288	66.040602
1455.908183	98.743664	66.045607
1455.350883	99.644339	66.050612
1454.299239	100.860115	66.055617
1453.642940	91.733456	66.060622
1452.990287	85.151285	66.065626
1451.792858	97.626987	66.070631
1451.464525	91.543593	66.075636
1450.914413	97.087000	66.080641
1450.380582	94.092237	66.085646
1449.680955	92.957723	66.090650
1448.569547	102.294406	66.095655
1448.458963	98.764042	66.100660
1447.866437	97.257710	66.105665
1447.231676	92.140758	66.110670
1446.324481	100.360098	66.115674
1445.439918	99.108330	66.120679
1445.247097	96.753189	66.125684
1444.287990	101.153725	66.130689
1443.432928	98.640505	66.135694
1442.634861	103.434893	66.140698
1442.440127	105.843773	66.145703
1442.151524	91.078140	66.150708
1441.053011	87.170246	66.155713
1440.348241	90.798689	66.160718
1439.911291	91.792195	66.165722
1439.231018	97.386253	66.170727
1438.663123	95.833433	66.175732
1437.792263	98.701421	66.180737
1437.277004	97.414610	66.185742
1436.039698	97.948736	66.190746
1434.984618	97.769538	66.195751
1434.672999	95.573621	66.200756
1433.961595	104.340557	66.205761
1433.503173	101.305427	66.210766
1433.471769	97.521218	66.215770
1432.885447	104.078004	66.220775
1432.423369	87.982267	66.225780
1431.180113	99.457643	66.230785
1430.707645	92.290202	66.235790
1429.842202	95.709234	66.240794
1428.443211	102.552880	66.245799
1428.351626	93.826873	66.250804
1427.832642	93.275477	66.255809
1427.445712	97.920943	66.260814
1426.772217	85.895595	66.265818
1425.543197	90.141928	66.270823
1425.423212	99.642712	66.275828
1424.717791	103.755363	66.280833
1423.812768	95.884012	66.285838
1422.968061	90.275343	66.290842
1421.990600	105.354193	66.295847
1421.882850	98.182393	66.300852
1421.540987	94.103776	66.305857
1420.912327	86.127005	66.310862
1420.182019	93.255425	66.315866
1419.153438	103.340580	66.320871
1418.665304	85.244793	66.325876
1417.728682	94.302978	66.330881
1417.042737	98.112929	66.335886
1416.680503	92.671985	66.340890
1416.036649	91.626380	66.345895
1415.549584	85.571381	66.350900
1415.211522	89.401723	66.355905
1414.292740	88.207443	66.360910
1412.897174	88.858194	66.365914
1412.115054	88.359666	66.370919
1411.819161	95.278694	66.375924
1411.372527	100.539170	66.380929
1410.967529	102.245077	66.385934
1410.331689	96.538558	66.390938
1409.412055	99.166739	66.395943
1408.765042	90.557410	66.400948
1408.420913	89.341169	66.405953
1407.190948	93.404745	66.410958
1406.449884	93.375906	66.415962
1405.849568	101.464480	66.420967
1405.648485	86.287579	66.425972
1404.671500	92.767700	66.430977
1403.798882	91.182906	66.435982
1403.175986	96.297945	66.440986
1402.570282	105.130082	66.445991
1402.079540	95.417334	66.450996
1401.616417	93.464690	66.456001
1400.182116	106.495281	66.461006
1399.913110	95.037962	66.466010
1399.212242	99.889445	66.471015
1398.944123	95.770726	66.476020
1398.394187	89.580652	66.481025
1397.818037	97.069328	66.486030
1397.213984	91.655789	66.491034
1396.164053	94.662635	66.496039
1395.324475	92.080744	66.501044
1394.823292	86.445864	66.506049
1394.178027	98.852734	66.511054
1393.944014	93.916508	66.516058
1392.445638	98.126832	66.521063
1391.651179	91.696523	66.526068
1391.034856	101.195785	66.531073
1391.060507	96.541539	66.536078
1390.748700	81.760696	66.541082
1389.371735	88.066295	66.546087
1388.699401	89.445714	66.551092
1388.444926	92.586296	66.556097
1387.514518	85.097450	66.561102
1386.680394	87.350942	66.566106
1385.545115	103.856720	66.571111
1385.439377	86.241023	66.576116
1385.005602	98.185366	66.581121
1384.316381	94.184050	66.586126
1384.202910	96.966346	66.591130
1383.176817	98.723684	66.596135
1382.389722	95.475901	66.601140
1381.321793	89.346099	66.606145
1380.264569	100.486009	66.611150
1380.070308	96.730845	66.616154
1379.205075	100.310701	66.621159
1379.009196	94.669863	66.626164
1378.474943	100.174493	66.631169
1377.984798	108.286560	66.636174
1377.171661	89.367288	66.641178
1376.322066	94.696555	66.646183
1376.066318	95.461004	66.651188
1375.084494	95.948238	66.656193
1374.031646	86.890957	66.661198
1374.072723	90.476537	66.666202
1373.216271	98.785595	66.671207
1372.022454	83.266655	66.676212
1371.754992	80.093959	66.681217
1370.947956	91.662421	66.686222
1370.716772	81.878469	66.691226
1369.481968	89.440315	66.696231
1368.966181	82.519465	66.701236
1368.582894	95.531203	66.706241
1368.069753	88.945802	66.711246
1366.987243	92.678465	66.716250
1366.208438	95.607530	66.721255
1365.938336	83.434506	66.726260
1365.156553	89.024213	66.731265
1364.304620	88.710253	66.736270
1363.728872	88.365002	66.741274
1363.112986	99.247108	66.746279
1363.071168	75.935089	66.751284
1361.991522	93.982074	66.756289
1360.430968	89.406544	66.761294
1360.454716	85.768107	66.766298
1359.736839	90.658567	66.771303
1359.507563	84.832244	66.776308
1358.564280	102.726683	66.781313
1357.641418	93.407482	66.786318
1357.616376	86.211508	66.791322
1356.163146	94.516099	66.796327
1355.376759	93.529438	66.801332
1354.828118	88.739427	66.806337
1354.467209	92.076695	66.811342
1354.401629	84.937627	66.816346
1353.331428	96.834923	66.821351
1352.202383	100.587606	66.826356
1351.776649	93.064269	66.831361
1351.432592	96.294785	66.836366
1350.919952	82.228664	66.841370
1349.670137	96.685383	66.846375
1349.191091	86.275400	66.851380
1348.844291	82.512957	66.856385
1347.958239	93.138407	66.861390
1347.172064	81.984092	66.866394
1346.301668	85.019179	66.871399
1346.103699	81.997855	66.876404
1345.531067	82.623461	66.881409
1344.096639	91.142674	66.886414
1343.826290	95.525199	66.891418
1343.337937	94.289322	66.896423
1342.941031	87.753254	66.901428
1342.242263	89.859091	66.906433
1341.112717	88.930145	66.911438
1340.479480	87.206399	66.916442
1339.550681	102.561363	66.921447
1339.700640	94.243220	66.926452
1338.583324	89.070564	66.931457
1337.830727	89.718476	66.936462
1337.302392	92.074747	66.941466
1336.809323	99.878212	66.946471
1336.147940	90.627832	66.951476
1335.559687	95.152357	66.956481
1335.228066	88.277925	66.961486
1334.326255	88.824988	66.966490
1332.807552	94.441984	66.971495
1332.647731	88.806460	66.976500
1332.383910	83.952252	66.981505
1331.466674	104.799177	66.986510
1330.829300	90.199407	66.991514
1329.606854	80.812745	66.996519
1329.325150	95.626456	67.001524
1328.973068	81.971608	67.006529
1328.423750	85.184298	67.011534
1327.565213	77.247265	67.016538
1326.514805	91.692783	67.021543
1326.217468	96.115868	67.026548
1325.740576	94.340460	67.031553
1324.613744	85.785373	67.036558
1324.528112	84.263134	67.041562
1323.511546	109.438582	67.046567
1322.492711	81.669567	67.051572
1322.001686	91.412247	67.056577
1321.423716	95.320163	67.061582
1321.120048	84.565357	67.066586
1320.358517	96.415163	67.071591
1319.573837	86.334464	67.076596
1319.158195	91.560059	67.081601
1318.219458	78.190868	67.086606
1317.494928	82.957821	67.091610
1316.800612	89.665823	67.096615
1316.346580	82.429258	67.101620
1315.881659	92.932567	67.106625
1314.806253	100.150571	67.111630
1314.085387	89.477863	67.116634
1313.620802	88.949378	67.121639
1313.078566	90.199328	67.126644
1311.817202	87.968364	67.131649
1311.341039	91.360228	67.136654
1310.557253	86.200786	67.141658
1310.215480	94.178881	67.146663
1309.857857	96.430749	67.151668
1309.407509	89.843264	67.156673
1308.558167	95.418500	67.161678
1308.076822	93.667457	67.166682
1306.588853	89.093037	67.171687
1305.894072	84.195396	67.176692
1305.605542	85.256784	67.181697
1304.939497	98.169987	67.186702
1304.757327	89.269178	67.191706
1303.491412	97.148221	67.196711
1302.629675	93.056095	67.201716
1301.984787	88.806497	67.206721
1301.099369	89.008787	67.211726
1301.361613	86.469350	67.216730
1300.799256	92.874116	67.221735
1299.933479	93.689836	67.226740
1299.277853	98.294464	67.231745
1298.356917	102.770976	67.236750
1297.612958	78.890981	67.241754
1296.448506	86.793309	67.246759
1295.928927	102.762844	67.251764
1295.895536	91.507774	67.256769
1295.528611	96.758741	67.261774
1294.915157	76.530520	67.266778
1293.642843	107.251461	67.271783
1293.524525	94.563906	67.276788
1292.806450	92.224491	67.281793
1291.489335	94.201592	67.286798
1290.934977	86.689263	67.291802
1290.479239	90.841085	67.296807
1289.951475	96.322619	67.301812
1288.777022	89.117033	67.306817
1287.980450	94.851031	67.311822
1288.236137	93.534704	67.316826
1287.541252	94.512480	67.321831
1286.503367	89.202647	67.326836
1285.590055	93.408304	67.331841
1284.821001	105.178900	67.336846
1284.692470	89.392857	67.341850
1283.909688	94.713102	67.346855
1283.215894	91.592436	67.351860
1282.376328	90.652099	67.356865
1281.739886	96.671280	67.361870
1281.710392	83.234795	67.366874
1280.643069	89.760853	67.371879
1280.197911	90.943337	67.376884
1279.527196	79.521550	67.381889
1278.026535	92.166937	67.386894
1277.747406	79.691038	67.391898
1276.913570	84.987862	67.396903
1276.658867	88.782885	67.401908
1276.152932	76.756191	67.406913
1275.244934	94.697060	67.411918
1274.359394	91.007678	67.416922
1273.693026	87.291331	67.421927
1273.352490	98.489188	67.426932
1273.226222	82.389000	67.431937
1272.055132	92.605654	67.436942
1271.294708	85.838841	67.441946
1270.877472	84.407177	67.446951
1269.919924	93.847175	67.451956
1268.903182	83.959509	67.456961
1268.358312	89.467416	67.461966
1267.978240	78.817811	67.466970
1267.679398	93.763544	67.471975
1266.784300	84.808962	67.476980
1265.851046	94.648775	67.481985
1265.284808	91.047387	67.486990
1265.253482	83.491321	67.491994
1263.660456	87.652111	67.496999
1263.299898	88.959908	67.502004
1262.897144	80.488404	67.507009
1262.330305	87.106763	67.512014
1261.394113	84.100339	67.517018
1260.340147	87.968844	67.522023
1259.728319	82.862497	67.527028
1259.434819	81.688688	67.532033
1259.068355	82.669437	67.537038
1258.194317	82.772166	67.542042
1257.183717	87.866882	67.547047
1256.734802	93.618141	67.552052
1256.368146	79.415308	67.557057
1255.242850	96.029903	67.562062
1254.585844	81.367066	67.567066
1253.804163	84.656141	67.572071
1253.491539	85.224653	67.577076
1253.071717	79.121161	67.582081
1252.012443	85.554490	67.587086
1251.694503	83.033197	67.592090
1250.602074	88.308075	67.597095
1250.223146	85.911591	67.602100
1249.264121	80.463090	67.607105
1248.341590	80.430039	67.612110
1248.130994	85.605687	67.617114
1247.604401	87.698361	67.622119
1247.022739	88.380615	67.627124
1246.749942	85.609306	67.632129
1245.600740	90.872716	67.637134
1245.070795	86.291062	67.642138
1244.093994	92.966734	67.647143
1243.100455	88.471416	67.652148
1242.713039	79.147549	67.657153
1242.204689	91.411240	67.662158
1241.948344	74.256333	67.667162
1240.807908	84.258394	67.672167
1240.268300	78.863042	67.677172
1239.816392	82.419783	67.682177
1238.888806	88.901558	67.687182
1238.607272	69.664473	67.692186
1237.167772	107.984098	67.697191
1236.875251	92.394443	67.702196
1236.802713	82.263609	67.707201
1235.863290	92.467088	67.712206
1235.036535	86.179164	67.717210
1234.320958	96.000139	67.722215
1233.680390	90.026363	67.727220
1233.076030	76.883148	67.732225
1232.207217	93.471150	67.737230
1231.772563	83.309598	67.742234
1231.210126	85.308631	67.747239
1230.105965	91.265012	67.752244
1229.505139	82.080735	67.757249
1228.746060	88.497871	67.762254
1228.793873	87.999875	67.767258
1227.872831	95.827257	67.772263
1226.775296	80.018727	67.777268
1226.218317	84.926204	67.782273
1225.633356	90.123545	67.787278
1225.420420	75.983006	67.792282
1224.284141	87.944453	67.797287
1223.609987	89.582808	67.802292
1223.534454	84.619831	67.807297
1222.805632	90.448719	67.812302
1221.731985	81.855271	67.817306
1220.962435	81.290152	67.822311
1220.399940	84.063436	67.827316
1219.895329	85.211232	67.832321
1218.698032	88.139083	67.837326
1218.042493	83.285691	67.842330
1217.716245	91.614536	67.847335
1217.260258	85.362268	67.852340
1217.074867	90.193309	67.857345
1215.968905	89.142404	67.862350
1215.405501	79.701461	67.867354
1214.681272	96.591310	67.872359
1213.417795	91.498727	67.877364
1212.862538	82.732961	67.882369
1212.028217	89.975728	67.887374
1211.994253	81.485009	67.892378
1211.675752	97.911389	67.897383
1210.743754	90.932199	67.902388
1210.059289	71.759201	67.907393
1209.055926	98.621362	67.912398
1208.732291	81.352585	67.917402
1207.757758	99.840185	67.922407
1206.937673	87.418790	67.927412
1206.733418	78.747009	67.932417
1205.961567	89.844731	67.937422
1205.381785	77.418243	67.942426
1204.267707	85.093409	67.947431
1203.494661	104.212830	67.952436
1203.839839	90.901257	67.957441
1202.713902	87.461435	67.962446
1202.125542	80.623134	67.967450
1201.384102	89.642447	67.972455
1200.996733	92.192353	67.977460
1199.748772	95.976624	67.982465
1199.202423	78.133028	67.987470
1198.480682	112.432634	67.992474
1198.011627	72.831805	67.997479
1197.224924	105.266838	68.002484
1196.251308	81.625259	68.007489
1195.783522	100.789163	68.012494
1195.313987	81.742816	68.017498
1195.002915	106.162713	68.022503
1194.387372	84.220809	68.027508
1193.614082	83.362997	68.032513
1192.995931	99.434935	68.037518
1192.062337	76.491860	68.042522
1191.199580	92.340934	68.047527
1190.663608	98.449803	68.052532
1190.484542	78.272384	68.057537
1189.221239	102.350161	68.062542
1188.116133	72.483559	68.067546
1187.533093	95.445521	68.072551
1187.087725	80.685979	68.077556
1186.678882	91.688127	68.082561
1186.492823	107.497399	68.087566
1186.188490	73.447746	68.092570
1184.949202	100.820494	68.097575
1184.192142	86.596194	68.102580
1183.518639	91.878583	68.107585
1182.498144	79.364509	68.112590
1182.184217	90.200181	68.117594
1181.635467	88.483538	68.122599
1180.957494	88.794793	68.127604
1180.086208	85.478475	68.132609
1179.290261	87.500466	68.137614
1178.918748	83.453418	68.142618
1178.513037	98.414573	68.147623
1177.239022	91.839857	68.152628
1176.691922	80.224994	68.157633
1175.976974	93.262673	68.162638
1175.920595	84.083278	68.167642
1175.134750	99.929592	68.172647
1173.986770	74.532339	68.177652
1173.581922	92.539844	68.182657
1173.121305	91.670152	68.187662
1172.131651	74.020075	68.192666
1171.409393	101.264864	68.197671
1170.327725	99.864782	68.202676
1170.641696	86.048850	68.207681
1169.983091	97.333564	68.212686
1168.960922	78.845033	68.217690
1168.207559	83.294926	68.222695
1167.660339	101.009714	68.227700
1167.051619	90.585717	68.232705
1165.794127	91.326597	68.237710
1165.154389	93.866189	68.242714
1165.057720	96.220063	68.247719
1164.476616	92.871786	68.252724
1164.129148	87.117905	68.257729
1162.961335	83.246396	68.262734
1162.665565	83.968347	68.267738
1161.772857	91.004384	68.272743
1160.940611	98.666284	68.277748
1160.135532	81.885658	68.282753
1159.499892	108.586859	68.287758
1159.567528	78.637811	68.292762
1158.343067	104.950140	68.297767
1157.429209	97.031428	68.302772
1157.020522	88.124099	68.307777
1156.404736	102.093710	68.312782
1155.794606	101.929007	68.317786
1154.921946	96.605568	68.322791
1154.188760	74.315002	68.327796
1154.020718	91.360800	68.332801
1152.942768	90.724912	68.337806
1152.087254	84.206645	68.342810
1151.799670	91.130667	68.347815
1151.229025	91.207252	68.352820
1150.892166	92.949662	68.357825
1149.734916	91.194203	68.362830
1149.422684	84.099120	68.367834
1148.809565	85.413989	68.372839
1147.682208	91.000373	68.377844
1147.064959	86.208717	68.382849
1146.468144	91.925167	68.387854
1146.351627	95.901635	68.392858
1144.957822	83.754444	68.397863
1143.921483	89.496652	68.402868
1143.772706	89.129267	68.407873
1143.393580	95.526989	68.412878
1142.741685	87.557160	68.417882
1141.815281	90.762060	68.422887
1141.021132	74.302971	68.427892
1140.918075	85.124021	68.432897
1139.570206	97.530718	68.437902
1138.835309	95.905191	68.442906
1138.297869	84.742938	68.447911
1138.098390	90.035087	68.452916
1137.371058	98.001984	68.457921
1136.636872	72.420678	68.462926
1135.746038	105.958730	68.467930
1134.946691	81.340199	68.472935
1134.750192	86.456842	68.477940
1134.079801	81.820292	68.482945
1132.965033	102.552011	68.487950
1132.141954	97.826209	68.492954
1132.094804	63.554359	68.497959
1131.330761	65.926079	68.502964
1131.010827	100.270540	68.507969
1129.622116	110.964970	68.512974
1129.313708	88.245726	68.517978
1128.809983	84.226026	68.522983
1128.095997	108.557051	68.527988
1127.621662	91.574018	68.532993
1126.352039	90.203854	68.537998
1126.322232	84.733746	68.543002
1125.117474	95.868811	68.548007
1124.453630	85.095654	68.553012
1123.891531	77.346506	68.558017
1123.262576	105.924676	68.563022
1123.156145	86.602986	68.568026
1122.090830	81.423746	68.573031
1121.076994	94.791235	68.578036
1120.551110	97.166078	68.583041
1119.985815	86.858189	68.588046
1119.429513	89.535896	68.593050
1118.568435	98.574261	68.598055
1117.783464	83.886106	68.603060
1117.928908	84.531570	68.608065
1116.741714	91.441009	68.613070
1116.160188	72.954960	68.618074
1115.294606	98.130049	68.623079
1114.869942	77.734693	68.628084
1114.647423	82.098580	68.633089
1113.261396	99.497392	68.638094
1112.560483	79.390391	68.643098
1111.832564	84.738215	68.648103
1111.645320	101.250941	68.653108
1110.652674	73.347047	68.658113
1110.015906	107.663076	68.663118
1109.388062	96.289713	68.668122
1109.268754	94.022255	68.673127
1108.170224	94.783606	68.678132
1107.455572	85.015114	68.683137
1106.576789	99.337204	68.688142
1106.194532	87.122161	68.693146
1105.988847	79.612770	68.698151
1104.660188	84.467990	68.703156
1104.379609	86.494748	68.708161
1103.592633	94.767587	68.713166
1103.126096	85.901014	68.718170
1102.062824	77.244483	68.723175
1101.369170	87.061987	68.728180
1101.568065	87.744677	68.733185
1099.934257	76.138720	68.738190
1098.865885	100.614411	68.743194
1098.825651	91.154925	68.748199
1098.002327	92.679854	68.753204
1098.271186	90.670751	68.758209
1097.360913	94.018171	68.763214
1096.427190	84.029082	68.768218
1095.903994	84.329930	68.773223
1094.745472	94.486303	68.778228
1093.865042	86.678996	68.783233
1093.134607	101.557776	68.788238
1092.966355	92.424567	68.793242
1092.987996	76.449123	68.798247
1091.574150	81.265863	68.803252
1090.808311	89.175815	68.808257
1090.251072	95.928286	68.813262
1089.672370	79.523247	68.818266
1089.280794	89.543421	68.823271
1088.065231	103.930133	68.828276
1087.651945	94.265079	68.833281
1087.410920	90.235133	68.838286
1086.612877	90.679048	68.843290
1085.557965	99.864945	68.848295
1084.931961	92.061316	68.853300
1084.707745	76.798304	68.858305
1083.455256	93.374831	68.863310
1082.736176	94.225630	68.868314
1082.190758	91.157111	68.873319
1081.731069	90.585316	68.878324
1081.433915	84.389812	68.883329
1080.534168	76.289140	68.888334
1079.877255	91.225597	68.893338
1079.599696	81.948945	68.898343
1078.271502	80.919265	68.903348
1077.483118	97.738915	68.908353
1076.835327	84.648391	68.913358
1076.275811	93.080580	68.918362
1076.371045	89.317244	68.923367
1074.796187	77.307713	68.928372
1074.336367	79.446561	68.933377
1073.419010	85.106789	68.938382
1073.294653	86.826439	68.943386
1073.088254	97.797966	68.948391
1071.533435	95.072948	68.953396
1071.138392	81.967450	68.958401
1070.812120	89.616677	68.963406
1070.110209	77.543963	68.968410
1069.088334	92.536907	68.973415
1068.172769	97.391080	68.978420
1067.918266	77.340811	68.983425
1067.376019	92.445098	68.988430
1066.552786	82.367488	68.993434
1066.094217	73.373516	68.998439
1065.144993	95.856023	69.003444
1064.884114	86.712328	69.008449
1063.736053	82.033528	69.013454
1062.786403	79.207512	69.018458
1062.425173	91.608647	69.023463
1062.039806	76.872720	69.028468
1061.439100	79.767223	69.033473
1060.629407	88.813190	69.038478
1059.903483	85.989424	69.043482
1059.817046	77.280004	69.048487
1058.469568	100.193285	69.053492
1058.259781	87.260151	69.058497
1057.673424	86.993924	69.063502
1056.684647	75.479335	69.068506
1055.563226	96.103316	69.073511
1055.188165	83.718421	69.078516
1054.841785	81.688932	69.083521
1054.281600	85.702868	69.088526
1053.320127	92.850795	69.093530
1052.581038	82.819725	69.098535
1051.941770	85.447569	69.103540
1051.674892	79.247256	69.108545
1050.497033	85.250116	69.113550
1049.760653	84.126295	69.118554
1049.383318	84.489096	69.123559
1049.119126	73.608241	69.128564
1048.133825	82.898175	69.133569
1047.206706	95.576992	69.138574
1046.385012	77.168600	69.143578
1046.232115	68.360957	69.148583
1045.721037	88.318579	69.153588
1044.773555	82.398426	69.158593
1044.041562	81.475747	69.163598
1043.568209	83.247769	69.168602
1042.733769	87.895087	69.173607
1041.815196	79.639739	69.178612
1041.414723	90.356725	69.183617
1040.875413	78.904664	69.188622
1040.016145	82.852653	69.193626
1039.257164	80.806815	69.198631
1038.399614	79.694392	69.203636
1038.229887	74.139330	69.208641
1037.717455	90.006801	69.213646
1037.392290	75.072083	69.218650
1036.288917	72.297342	69.223655
1035.905168	83.672366	69.228660
1035.167607	72.087862	69.233665
1033.770686	70.717501	69.238670
1032.824681	92.988196	69.243674
1032.580988	52.334596	69.248679
1031.899143	84.366562	69.253684
1031.856960	87.788761	69.258689
1031.055289	84.945520	69.263694
1030.174554	81.318545	69.268698
1029.911097	89.169078	69.273703
1028.955445	80.336198	69.278708
1028.176448	105.000817	69.283713
1027.326011	83.941566	69.288718
1026.984602	79.434046	69.293722
1026.522893	90.242772	69.298727
1025.417244	84.248450	69.303732
1024.566795	71.270624	69.308737
1024.110025	77.081495	69.313742
1023.617064	88.880729	69.318746
1023.523228	94.510867	69.323751
1022.056526	84.655497	69.328756
1021.681905	82.878073	69.333761
1021.002845	84.799516	69.338766
1020.387381	86.212553	69.343770
1019.481400	80.131277	69.348775
1018.429193	97.748226	69.353780
1018.453609	75.704598	69.358785
1017.906221	77.866848	69.363790
1017.027883	84.340851	69.368794
1016.340670	84.429706	69.373799
1015.557729	86.735086	69.378804
1015.562688	78.712831	69.383809
1014.621198	81.964323	69.388814
1013.719068	81.235871	69.393818
1013.732958	84.415772	69.398823
1011.991622	85.227405	69.403828
1011.547770	79.566159	69.408833
1010.709080	76.110688	69.413838
1010.376644	85.277834	69.418842
1009.762934	86.577060	69.423847
1009.300764	62.928368	69.428852
1008.145997	84.577874	69.433857
1007.914947	84.816487	69.438862
1007.601099	83.141353	69.443866
1006.702615	76.959549	69.448871
1005.669570	83.004035	69.453876
1005.137157	78.629407	69.458881
1004.460852	67.845677	69.463886
1003.524483	85.092543	69.468890
1003.135053	73.063174	69.473895
1002.499778	70.609760	69.478900
1002.186334	60.304431	69.483905
1000.679367	84.603907	69.488910
1000.078183	76.264965	69.493914
999.585788	71.261114	69.498919
998.944459	89.752487	69.503924
999.039223	80.438687	69.508929
998.243101	74.426669	69.513934
997.337966	85.217646	69.518938
997.064542	78.589479	69.523943
995.541212	80.780875	69.528948
994.959382	76.537108	69.533953
994.183714	94.590998	69.538958
993.915090	88.737877	69.543962
993.806575	76.455664	69.548967
992.404879	82.962490	69.553972
991.757710	66.459598	69.558977
991.000766	95.118023	69.563982
990.819137	73.067770	69.568986
990.247990	62.559035	69.573991
988.761716	88.468353	69.578996
989.012845	70.961554	69.584001
988.316553	79.456509	69.589006
987.117568	91.713422	69.594010
986.804512	75.311890	69.599015
985.807846	74.062360	69.604020
985.756848	76.643917	69.609025
984.802740	76.451993	69.614030
983.772116	79.695602	69.619034
983.689986	77.520005	69.624039
982.696596	74.432916	69.629044
981.643024	66.727332	69.634049
980.912631	94.802825	69.639054
980.549233	81.137265	69.644058
980.087411	70.716781	69.649063
979.654766	78.524850	69.654068
978.664148	75.609199	69.659073
977.885801	74.372238	69.664078
977.382109	74.862382	69.669082
977.172236	73.382007	69.674087
976.118613	83.125930	69.679092
975.413869	83.510881	69.684097
974.938300	76.019231	69.689102
974.000704	79.358420	69.694106
973.134307	63.219988	69.699111
972.103895	83.585075	69.704116
971.581971	83.297577	69.709121
971.407570	75.680737	69.714126
971.061845	79.163850	69.719130
970.741303	73.544492	69.724135
969.530562	80.976516	69.729140
969.439615	71.157722	69.734145
968.048435	76.945413	69.739150
967.171305	79.601666	69.744154
966.749659	67.714625	69.749159
966.239558	71.178165	69.754164
965.675341	71.961777	69.759169
964.450864	76.169739	69.764174
963.857816	71.817388	69.769178
963.818014	75.989788	69.774183
963.253059	79.760085	69.779188
962.494345	68.070177	69.784193
961.541813	75.626683	69.789198
960.883822	71.420276	69.794202
959.918294	72.106911	69.799207
959.283100	80.344583	69.804212
958.906239	76.042979	69.809217
958.547892	77.066629	69.814222
957.814320	73.676447	69.819226
956.581964	70.769315	69.824231
955.455044	80.562751	69.829236
955.340090	68.196426	69.834241
954.905592	72.130455	69.839246
954.772911	82.916781	69.844250
954.064668	70.846704	69.849255
953.198370	88.128161	69.854260
952.531622	74.384741	69.859265
951.521926	66.683227	69.864270
950.518635	62.268442	69.869274
950.207998	73.852585	69.874279
949.777697	77.014865	69.879284
949.399505	72.297186	69.884289
948.599468	63.389131	69.889294
947.522901	73.004252	69.894298
947.403774	76.241584	69.899303
945.827307	81.300306	69.904308
945.484020	78.097162	69.909313
944.958923	74.120331	69.914318
944.441388	77.848394	69.919322
943.983316	74.912661	69.924327
942.715584	75.120725	69.929332
942.302766	69.751010	69.934337
941.889816	73.851912	69.939342
941.234441	75.096286	69.944346
940.332223	65.351415	69.949351
939.301732	79.409096	69.954356
938.695738	77.537629	69.959361
938.529433	61.428144	69.964366
937.738845	93.299242	69.969370
937.262064	70.543819	69.974375
936.416921	78.795983	69.979380
935.641998	72.738041	69.984385
935.513311	71.938567	69.989390
934.394736	78.001417	69.994394
933.741352	67.631934	69.999399
933.338959	86.675025	70.004404
932.771445	67.942420	70.009409
931.569683	69.078220	70.014414
930.816709	69.354171	70.019418
930.520820	65.455980	70.024423
930.052903	82.451697	70.029428
929.060831	76.108212	70.034433
928.015892	80.054244	70.039438
927.812990	76.778302	70.044442
927.468865	63.174359	70.049447
926.948864	68.266794	70.054452
926.024731	73.335243	70.059457
925.470919	86.410380	70.064462
924.773135	77.265293	70.069466
923.643361	62.737775	70.074471
922.862120	71.924304	70.079476
922.270433	75.055504	70.084481
922.102657	69.239968	70.089486
921.174356	62.135761	70.094490
920.622853	63.710517	70.099495
919.873216	73.850745	70.104500
919.806625	71.671102	70.109505
918.279991	66.585882	70.114510
917.432111	74.838483	70.119514
917.157789	69.200743	70.124519
916.628488	82.883797	70.129524
916.409512	71.242040	70.134529
915.549215	69.286481	70.139534
914.632563	71.786622	70.144538
914.127231	67.084456	70.149543
913.291232	78.381653	70.154548
912.326417	68.615218	70.159553
911.635658	79.821497	70.164558
910.805109	71.761926	70.169562
910.872511	58.100382	70.174567
910.380136	70.240115	70.179572
909.647312	84.029673	70.184577
908.887395	75.238237	70.189582
908.192608	61.682225	70.194586
907.542602	66.776431	70.199591
906.297299	72.440015	70.204596
905.780492	81.464627	70.209601
905.867828	63.543971	70.214606
904.421622	69.666857	70.219610
903.646009	66.168276	70.224615
903.191639	71.423724	70.229620
902.968637	73.329377	70.234625
902.603490	80.554313	70.239630
901.349560	75.263282	70.244634
900.770523	72.961784	70.249639
899.885348	72.400976	70.254644
899.700333	71.124798	70.259649
898.625792	70.840118	70.264654
898.015970	79.368632	70.269658
897.518536	77.003688	70.274663
897.051381	74.479392	70.279668
896.438343	71.828515	70.284673
895.399368	75.765725	70.289678
894.403976	68.043039	70.294682
894.382451	67.407851	70.299687
893.410706	75.760592	70.304692
892.450191	72.050183	70.309697
891.971418	71.093556	70.314702
891.382432	75.277672	70.319706
891.274445	73.448373	70.324711
890.282811	77.374897	70.329716
889.357331	81.153706	70.334721
888.956415	79.620173	70.339726
888.223218	72.527498	70.344730
887.877334	70.392309	70.349735
886.908679	69.191975	70.354740
886.217282	69.202688	70.359745
885.972999	74.979754	70.364750
884.544241	72.900231	70.369754
883.994394	64.778653	70.374759
883.390800	77.558953	70.379764
883.086683	71.460787	70.384769
882.611197	75.456540	70.389774
881.499999	82.737147	70.394778
881.358617	66.041845	70.399783
880.725031	77.336792	70.404788
879.813339	70.206303	70.409793
879.115014	83.239791	70.414798
878.351291	82.948224	70.419802
877.782212	74.355070	70.424807
876.191037	93.655183	70.429812
875.991412	79.974627	70.434817
875.804033	69.977242	70.439822
875.396435	76.157172	70.444826
874.699555	77.152718	70.449831
873.722715	73.671982	70.454836
873.149430	78.894328	70.459841
872.591670	71.713815	70.464846
871.403574	75.804071	70.469850
870.986053	76.039261	70.474855
870.351617	84.987990	70.479860
869.827184	73.036915	70.484865
868.694696	69.498960	70.489870
867.836408	71.751722	70.494874
867.648383	63.985695	70.499879
866.964925	74.353505	70.504884
866.771483	76.032120	70.509889
866.058467	81.779725	70.514894
865.098955	80.549560	70.519898
864.421528	70.680637	70.524903
864.155865	70.617285	70.529908
863.203731	75.523064	70.534913
862.157520	74.751373	70.539918
861.800441	77.328035	70.544922
861.561346	64.193064	70.549927
860.287883	65.605221	70.554932
859.766241	72.954406	70.559937
859.169326	74.541134	70.564942
858.447697	69.930177	70.569946
857.730095	62.928070	70.574951
856.755162	67.861130	70.579956
856.340936	69.347821	70.584961
855.994923	70.003690	70.589966
855.453433	76.570764	70.594970
854.753199	70.452083	70.599975
853.744275	75.042072	70.604980
853.135364	67.671026	70.609985
852.848253	72.964508	70.614990
851.773119	77.847295	70.619994
851.335764	71.171139	70.624999
850.773979	78.873627	70.630004
849.811684	84.495346	70.635009
849.012495	76.433961	70.640014
848.276800	78.395998	70.645018
848.341498	71.876455	70.650023
847.580537	71.368429	70.655028
846.063434	80.249515	70.660033
845.713396	66.045752	70.665038
845.287762	70.047764	70.670042
844.837025	73.798324	70.675047
843.937879	70.257928	70.680052
843.462955	74.846494	70.685057
842.764987	74.035147	70.690062
842.226431	67.591133	70.695066
841.629326	60.937260	70.700071
840.535192	62.631521	70.705076
839.926147	69.139965	70.710081
839.769578	68.114715	70.715086
838.301053	76.390442	70.720090
838.172221	69.159009	70.725095
837.092044	76.918786	70.730100
836.990287	74.359992	70.735105
836.207097	75.519089	70.740110
834.730534	93.561568	70.745114
834.689456	79.343306	70.750119
834.025228	83.052163	70.755124
833.637580	77.719461	70.760129
832.717828	74.639637	70.765134
831.573398	73.610798	70.770138
831.365934	85.497051	70.775143
831.304366	83.800706	70.780148
830.150447	82.347627	70.785153
829.631214	73.872702	70.790158
828.563580	75.080234	70.795162
828.382060	69.891331	70.800167
827.193679	77.471229	70.805172
826.440685	83.594192	70.810177
826.308855	72.277606	70.815182
825.682256	73.372357	70.820186
824.483560	75.622555	70.825191
823.597049	81.546012	70.830196
822.962815	86.819069	70.835201
823.000993	78.479326	70.840206
822.264301	85.870640	70.845210
821.974043	76.272813	70.850215
820.812774	78.668433	70.855220
820.303054	85.470141	70.860225
820.054772	82.666607	70.865230
818.701374	88.473591	70.870234
818.126916	74.830645	70.875239
817.608070	79.423054	70.880244
817.349735	80.744595	70.885249
816.294444	81.918630	70.890254
815.503065	83.318720	70.895258
815.194637	80.281925	70.900263
813.595920	86.184730	70.905268
812.694769	76.119640	70.910273
812.587301	72.364925	70.915278
812.000254	79.071714	70.920282
811.891370	71.288363	70.925287
811.030129	81.031671	70.930292
810.582293	81.793636	70.935297
809.697210	75.813197	70.940302
808.865171	74.669988	70.945306
808.610646	70.243292	70.950311
807.601881	70.173670	70.955316
806.781784	76.886022	70.960321
805.952755	78.616939	70.965326
805.679518	86.498992	70.970330
805.557743	76.032308	70.975335
804.319885	79.857719	70.980340
803.600649	84.412651	70.985345
803.318690	80.822899	70.990350
802.312487	78.165254	70.995354
801.663175	79.271512	71.000359
800.938620	78.325646	71.005364
800.636270	83.416571	71.010369
799.713213	77.041660	71.015374
798.954022	80.439234	71.020378
798.370956	73.795748	71.025383
798.025670	85.919969	71.030388
797.182404	87.080758	71.035393
796.144888	82.551642	71.040398
795.233554	86.858055	71.045402
795.191254	75.747978	71.050407
795.000437	76.073239	71.055412
794.058287	85.105658	71.060417
793.628714	76.800961	71.065422
792.084615	83.053028	71.070426
791.749103	84.096717	71.075431
790.930993	73.127496	71.080436
790.233636	79.210071	71.085441
790.129296	85.557763	71.090446
788.792847	76.014541	71.095450
788.174628	75.786565	71.100455
787.752473	80.962790	71.105460
787.553192	79.313600	71.110465
786.726391	77.847886	71.115470
785.479872	82.710679	71.120474
784.877365	78.452917	71.125479
784.431205	76.806764	71.130484
783.826816	85.282397	71.135489
783.701646	75.052786	71.140494
782.669218	90.131049	71.145498
781.782581	76.906799	71.150503
781.509004	84.142395	71.155508
780.569496	84.377129	71.160513
779.750665	79.541988	71.165518
778.999187	88.704897	71.170522
779.090235	75.547335	71.175527
778.039261	82.977654	71.180532
776.757860	84.030018	71.185537
776.566114	82.098950	71.190542
776.128656	87.060009	71.195546
775.610558	75.948418	71.200551
774.547141	76.351106	71.205556
773.934874	80.781787	71.210561
773.675922	68.351695	71.215566
772.214056	76.263718	71.220570
771.708392	72.258608	71.225575
771.219840	80.594381	71.230580
770.468890	86.560924	71.235585
770.473091	72.899984	71.240590
769.305343	83.314958	71.245594
768.582522	91.114059	71.250599
767.858210	59.211386	71.255604
767.415203	99.780257	71.260609
767.138313	76.281915	71.265614
765.965798	89.025088	71.270618
765.718113	71.889444	71.275623
764.462820	84.169583	71.280628
763.530455	92.274844	71.285633
763.116389	72.967553	71.290638
762.643624	75.945820	71.295642
762.027998	91.719350	71.300647
761.666134	87.133138	71.305652
760.860763	85.531564	71.310657
760.335813	77.484896	71.315662
759.617885	91.521254	71.320666
758.849443	91.996826	71.325671
757.930969	77.880425	71.330676
757.081077	89.458978	71.335681
756.818073	88.155807	71.340686
756.102286	89.102360	71.345690
755.494390	79.630807	71.350695
754.781785	81.937678	71.355700
754.103992	89.515161	71.360705
753.918678	81.589449	71.365710
753.016655	85.796627	71.370714
752.005050	80.785620	71.375719
751.612519	84.444932	71.380724
750.405065	83.681615	71.385729
749.929348	76.388732	71.390734
748.994060	87.840542	71.395738
748.970910	86.000897	71.400743
748.664843	94.429043	71.405748
748.023217	91.684989	71.410753
747.440984	77.943964	71.415758
746.237157	89.020665	71.420762
745.368703	80.702283	71.425767
744.435102	83.474824	71.430772
744.099051	92.918507	71.435777
743.729165	80.813560	71.440782
743.080581	84.945698	71.445786
742.027163	76.757688	71.450791
741.518308	88.865380	71.455796
740.993411	88.259880	71.460801
740.930505	84.952207	71.465806
739.651539	95.189377	71.470810
738.854195	76.688969	71.475815
738.666003	87.966639	71.480820
737.555376	91.230965	71.485825
736.743062	84.324391	71.490830
735.939366	85.346444	71.495834
735.687118	92.490346	71.500839
735.419233	80.134210	71.505844
733.897021	92.486826	71.510849
733.295717	91.693233	71.515854
732.481692	93.587355	71.520858
732.290068	85.397738	71.525863
732.247479	84.631872	71.530868
731.271512	87.562542	71.535873
730.310465	87.643039	71.540878
729.494139	84.412754	71.545882
729.324920	87.941901	71.550887
728.491555	92.027777	71.555892
727.356210	83.509061	71.560897
727.085761	83.701936	71.565902
726.489584	81.355905	71.570906
725.763024	82.827696	71.575911
724.709407	76.380573	71.580916
723.985106	89.251077	71.585921
724.501335	85.835423	71.590926
723.389806	95.579191	71.595930
722.483214	89.742548	71.600935
721.585380	80.517433	71.605940
721.191998	96.704987	71.610945
720.456939	85.183281	71.615950
719.533494	87.635690	71.620954
718.883185	92.089789	71.625959
718.620066	77.500075	71.630964
718.061739	89.429578	71.635969
717.162863	84.294987	71.640974
716.144653	90.934841	71.645978
716.008359	86.553979	71.650983
715.249144	95.636140	71.655988
714.337454	87.736211	71.660993
713.747450	74.888938	71.665998
713.149654	87.423928	71.671002
712.921293	91.752497	71.676007
711.441155	83.925740	71.681012
710.709226	86.251468	71.686017
710.295997	91.840997	71.691022
710.110635	74.211348	71.696026
709.742524	84.238836	71.701031
708.622183	87.777516	71.706036
707.689184	88.788629	71.711041
707.498599	77.845669	71.716046
706.779849	84.912472	71.721050
706.253706	86.399662	71.726055
705.659115	76.855052	71.731060
704.495321	87.059700	71.736065
703.617615	91.936340	71.741070
703.190434	96.488946	71.746074
702.936077	82.244744	71.751079
702.190729	90.165710	71.756084
700.792196	92.121378	71.761089
700.650083	78.075337	71.766094
699.723781	83.830136	71.771098
699.446486	87.076891	71.776103
698.998864	86.842271	71.781108
698.092112	79.029871	71.786113
697.441990	71.018927	71.791118
697.018703	83.272253	71.796122
695.881798	83.691406	71.801127
695.195775	85.678690	71.806132
694.433040	81.764991	71.811137
694.639577	81.066683	71.816142
693.401707	82.750782	71.821146
692.374673	85.758978	71.826151
691.948789	90.868007	71.831156
691.484973	89.300371	71.836161
690.678403	79.048399	71.841166
689.758612	87.377165	71.846170
689.157666	85.106015	71.851175
688.901329	85.004929	71.856180
688.418003	95.743010	71.861185
687.616252	79.452499	71.866190
686.661403	81.715967	71.871194
686.371337	78.447625	71.876199
685.479637	78.800930	71.881204
684.352447	85.618985	71.886209
684.084406	81.060425	71.891214
683.386771	84.695794	71.896218
683.135643	85.355499	71.901223
682.303796	86.339476	71.906228
681.026813	84.543388	71.911233
680.995970	80.809595	71.916238
680.307845	79.928922	71.921242
679.329462	83.389817	71.926247
678.449142	76.438910	71.931252
677.871355	92.196960	71.936257
677.816873	83.573955	71.941262
677.249693	88.199315	71.946266
676.198509	79.878525	71.951271
675.461032	84.732840	71.956276
674.755145	78.734959	71.961281
674.578803	74.656931	71.966286
673.114354	88.107324	71.971290
672.616043	93.264156	71.976295
672.228269	77.729271	71.981300
671.573075	84.994105	71.986305
671.381997	85.980118	71.991310
670.145586	85.776504	71.996314
669.958855	82.646240	72.001319
669.306157	81.212761	72.006324
667.808226	91.208878	72.011329
667.438953	84.666990	72.016334
666.883122	89.432462	72.021338
666.476320	83.017969	72.026343
665.622200	92.003295	72.031348
664.570639	74.524215	72.036353
664.656491	80.234526	72.041358
663.715640	89.905401	72.046362
663.105189	86.177183	72.051367
662.574805	79.548999	72.056372
661.778373	85.037139	72.061377
661.276664	84.304969	72.066382
659.906896	82.790157	72.071386
659.579394	82.061782	72.076391
659.089093	83.790839	72.081396
658.494706	93.991556	72.086401
657.980955	84.388355	72.091406
656.781700	88.510443	72.096410
656.005080	78.832422	72.101415
656.011235	74.550302	72.106420
655.134197	91.226430	72.111425
654.544226	78.729233	72.116430
653.919163	86.104382	72.121434
653.243796	78.436492	72.126439
652.684081	84.241728	72.131444
651.551252	77.819869	72.136449
651.073243	78.236606	72.141454
650.432453	88.499900	72.146458
649.528233	87.216862	72.151463
648.758633	85.466136	72.156468
647.953304	89.758868	72.161473
647.986031	82.214738	72.166478
647.373916	77.417686	72.171482
646.544422	78.872778	72.176487
645.422250	76.115406	72.181492
644.882065	84.442071	72.186497
644.762189	72.563832	72.191502
644.209032	83.284645	72.196506
643.120585	91.119925	72.201511
642.561196	77.996582	72.206516
642.057759	77.524872	72.211521
641.420136	79.354660	72.216526
640.425987	89.866607	72.221530
639.715561	86.094397	72.226535
639.298610	86.551871	72.231540
638.397937	87.408061	72.236545
637.777570	79.149558	72.241550
637.089695	81.925577	72.246554
636.537373	91.427357	72.251559
636.093239	89.925980	72.256564
635.049642	94.029597	72.261569
634.839103	90.051626	72.266574
634.319077	91.329712	72.271578
633.564993	81.000023	72.276583
632.294314	78.988506	72.281588
631.380519	91.165430	72.286593
631.428114	79.585346	72.291598
630.942708	85.151685	72.296602
629.879699	90.368498	72.301607
629.313659	80.007286	72.306612
628.634540	83.146164	72.311617
628.072064	84.658078	72.316622
626.885976	90.195673	72.321626
626.150723	87.157503	72.326631
626.054432	86.427000	72.331636
625.308812	95.402941	72.336641
625.172664	83.546210	72.341646
624.189621	88.510607	72.346650
623.331012	91.138792	72.351655
622.778747	80.910997	72.356660
622.077562	84.241037	72.361665
620.974600	82.281657	72.366670
620.433282	86.308434	72.371674
620.056472	87.688284	72.376679
619.960264	84.373308	72.381684
618.966380	91.023511	72.386689
618.526184	83.643008	72.391694
617.679438	91.778824	72.396698
616.546948	88.993147	72.401703
615.857361	88.363445	72.406708
615.365287	86.855516	72.411713
615.046615	87.708900	72.416718
614.090056	88.413160	72.421722
613.080247	87.202142	72.426727
612.807146	84.364743	72.431732
612.069309	86.590521	72.436737
611.699841	85.512468	72.441742
610.837804	83.591985	72.446746
609.859718	78.738122	72.451751
609.612232	75.319518	72.456756
609.115994	103.581639	72.461761
608.248654	83.830956	72.466766
607.579904	84.982933	72.471770
606.639408	83.622116	72.476775
606.546175	86.910520	72.481780
605.157382	81.781473	72.486785
604.515421	90.449188	72.491790
603.929730	76.740308	72.496794
603.793229	87.643908	72.501799
603.278339	85.020051	72.506804
602.125654	85.894317	72.511809
601.453391	75.155824	72.516814
601.147017	82.082854	72.521818
600.231610	78.529376	72.526823
599.680972	75.846565	72.531828
598.624460	95.015909	72.536833
598.312999	87.469834	72.541838
597.764657	70.224443	72.546842
596.619176	94.773978	72.551847
596.100467	73.323131	72.556852
595.687136	80.828556	72.561857
595.208464	80.086424	72.566862
593.962914	91.095715	72.571866
593.221978	85.847716	72.576871
593.255788	77.877669	72.581876
592.598350	95.286761	72.586881
591.951211	84.769753	72.591886
591.027887	83.445628	72.596890
590.205436	89.549751	72.601895
589.730177	81.198770	72.606900
588.974952	86.541603	72.611905
588.076252	81.224125	72.616910
587.424673	84.863219	72.621914
586.990395	82.234411	72.626919
587.121759	84.241329	72.631924
585.695118	96.085242	72.636929
584.670622	101.426819	72.641934
584.593726	78.751341	72.646938
584.062354	75.327499	72.651943
582.972295	99.901332	72.656948
581.947374	83.729989	72.661953
582.353298	69.114174	72.666958
580.992685	103.025058	72.671962
580.152433	77.025750	72.676967
580.006941	85.563928	72.681972
579.066020	83.908319	72.686977
578.295778	76.348603	72.691982
577.389698	84.785594	72.696986
576.661126	86.828568	72.701991
576.357349	86.208381	72.706996
575.879432	83.193891	72.712001
575.830059	69.363333	72.717006
574.793014	80.274760	72.722010
574.338712	85.861382	72.727015
573.522584	85.004282	72.732020
572.185362	91.002761	72.737025
571.726693	89.661397	72.742030
571.404610	78.584878	72.747034
570.369268	82.037538	72.752039
569.794533	79.074739	72.757044
568.862291	89.028101	72.762049
568.627979	79.323653	72.767054
567.971517	70.783943	72.772058
567.038931	82.512888	72.777063
566.636108	74.230798	72.782068
565.607033	78.103480	72.787073
565.378378	78.324406	72.792078
564.743333	86.659885	72.797082
563.671497	87.555980	72.802087
563.133408	77.179303	72.807092
562.610357	82.229708	72.812097
562.306817	80.065750	72.817102
560.929834	82.390197	72.822106
560.092098	81.120256	72.827111
560.023767	80.003704	72.832116
559.328075	85.367022	72.837121
558.898215	81.113360	72.842126
557.738940	76.529641	72.847130
557.334162	77.417246	72.852135
556.896445	76.450993	72.857140
556.141191	78.419378	72.862145
555.187093	68.638798	72.867150
554.678465	76.529964	72.872154
554.145867	82.539039	72.877159
553.516459	71.320686	72.882164
552.467442	82.145725	72.887169
551.908046	79.475358	72.892174
551.522735	75.541011	72.897178
550.881290	70.256686	72.902183
550.046577	80.524073	72.907188
549.178322	81.233213	72.912193
548.963186	78.266750	72.917198
548.255328	73.805081	72.922202
546.692390	80.821900	72.927207
546.618837	77.768233	72.932212
546.178532	78.311438	72.937217
545.616411	84.738353	72.942222
544.713721	72.352515	72.947226
543.818893	82.569561	72.952231
543.696135	73.971645	72.957236
542.841778	79.565230	72.962241
542.339250	83.213704	72.967246
541.291878	78.123344	72.972250
540.696057	70.330871	72.977255
540.320572	92.222180	72.982260
539.495220	79.779867	72.987265
538.966144	81.773724	72.992270
538.331435	79.930590	72.997274
537.597567	85.391450	73.002279
536.896229	83.465895	73.007284
535.893951	81.586704	73.012289
535.505993	84.196706	73.017294
535.390112	83.674318	73.022298
533.924076	89.499382	73.027303
533.134567	84.419982	73.032308
532.710687	87.253313	73.037313
532.331722	84.877461	73.042318
531.788804	84.476715	73.047322
531.017579	89.911993	73.052327
530.433801	83.656603	73.057332
529.799082	88.051490	73.062337
528.910595	86.346549	73.067342
528.367915	83.140549	73.072346
527.383755	88.407912	73.077351
527.480571	79.830207	73.082356
525.768008	85.968918	73.087361
525.315747	76.392235	73.092366
524.945310	80.842784	73.097370
524.265187	87.534491	73.102375
523.708453	83.474501	73.107380
522.614421	85.231956	73.112385
521.851153	81.154411	73.117390
521.473297	72.218695	73.122394
521.009574	83.726312	73.127399
520.902184	75.286790	73.132404
519.422341	89.950724	73.137409
519.206502	83.193628	73.142414
518.735863	86.710879	73.147418
517.464588	81.096416	73.152423
516.968433	74.002384	73.157428
516.436829	92.282351	73.162433
515.867491	81.495953	73.167438
515.004924	77.620298	73.172442
514.130273	88.365539	73.177447
513.621609	81.762320	73.182452
513.293896	83.129632	73.187457
512.568357	76.177792	73.192462
511.416295	83.452429	73.197466
510.839771	89.746037	73.202471
510.207875	75.219863	73.207476
509.999372	79.546851	73.212481
509.500611	75.211144	73.217486
508.900331	89.175176	73.222490
508.147270	75.912440	73.227495
507.009321	76.645638	73.232500
506.168120	82.371169	73.237505
505.535281	73.004601	73.242510
505.650856	85.260391	73.247514
504.508210	80.822273	73.252519
504.071869	70.642285	73.257524
503.403566	81.761476	73.262529
502.206273	77.612746	73.267534
501.273302	73.366717	73.272538
500.844661	83.566270	73.277543
500.472150	69.085509	73.282548
500.007654	80.642131	73.287553
499.699763	71.737849	73.292558
498.807340	71.372292	73.297562
497.872795	81.866894	73.302567
497.439486	80.677614	73.307572
496.340831	77.446666	73.312577
495.545607	80.132596	73.317582
495.676581	82.593701	73.322586
494.606571	80.331106	73.327591
494.116369	75.432681	73.332596
493.037314	84.430228	73.337601
492.555192	73.458072	73.342606
491.891470	76.490457	73.347610
490.700109	77.060295	73.352615
490.342496	67.151604	73.357620
489.674895	71.151213	73.362625
489.610377	66.776291	73.367630
488.888682	72.673583	73.372634
487.664264	81.489298	73.377639
487.523414	64.663131	73.382644
486.792564	84.449184	73.387649
486.263830	83.778123	73.392654
485.321053	73.620481	73.397658
484.721850	84.883199	73.402663
484.326578	76.628309	73.407668
482.882382	76.077873	73.412673
482.286135	77.951565	73.417678
481.879681	73.101299	73.422682
481.415723	66.694386	73.427687
481.086268	64.662296	73.432692
479.880962	75.422372	73.437697
479.293556	70.079000	73.442702
479.014131	67.386124	73.447706
477.660512	75.025598	73.452711
476.939626	67.478562	73.457716
476.154700	71.980960	73.462721
475.601543	76.354976	73.467726
475.753117	59.889053	73.472730
475.371009	74.840111	73.477735
474.414586	68.230983	73.482740
473.299744	71.339976	73.487745
472.959485	64.769866	73.492750
472.322640	70.335118	73.497754
471.176085	74.718528	73.502759
470.627481	73.456166	73.507764
470.288568	75.941675	73.512769
469.459291	66.414046	73.517774
468.423749	65.205615	73.522778
467.567255	83.385957	73.527783
467.409664	63.632679	73.532788
466.862597	74.846087	73.537793
466.739901	74.886147	73.542798
465.571143	79.730384	73.547802
464.520029	77.531020	73.552807
464.574757	69.846218	73.557812
463.737217	75.356724	73.562817
462.957389	69.788567	73.567822
462.268550	66.763560	73.572826
461.439301	79.437941	73.577831
460.693311	65.724707	73.582836
459.690602	77.682452	73.587841
459.503324	75.831124	73.592846
459.266579	66.417235	73.597850
458.609622	71.764936	73.602855
457.429240	73.392682	73.607860
456.905236	80.510502	73.612865
456.420661	73.455640	73.617870
455.649302	71.131288	73.622874
454.557847	77.219959	73.627879
454.185071	69.499202	73.632884
453.936054	77.462548	73.637889
453.131588	77.294291	73.642894
452.260125	71.505788	73.647898
451.616483	82.592674	73.652903
451.180056	74.041597	73.657908
450.064187	70.379783	73.662913
449.021836	64.941766	73.667918
448.523946	65.790610	73.672922
448.024994	76.871784	73.677927
447.995832	69.447915	73.682932
447.363797	70.367017	73.687937
446.684465	72.763276	73.692942
446.184852	78.699305	73.697946
445.092182	84.283585	73.702951
444.247582	74.815170	73.707956
443.810481	77.172834	73.712961
443.355884	75.256876	73.717966
442.600504	88.241174	73.722970
441.363304	83.819731	73.727975
441.305327	70.801066	73.732980
440.521283	75.516209	73.737985
439.640040	80.976921	73.742990
439.027486	80.762321	73.747994
438.186311	68.625340	73.752999
437.927636	70.333296	73.758004
436.746331	77.331940	73.763009
435.866612	78.060291	73.768014
435.343664	83.705172	73.773018
434.426240	83.703143	73.778023
434.476166	72.196828	73.783028
433.937849	72.817167	73.788033
433.653716	76.170678	73.793038
433.023818	76.419283	73.798042
431.835577	86.604270	73.803047
431.668105	75.734949	73.808052
430.205052	71.377887	73.813057
429.656918	73.354302	73.818062
429.143013	75.184925	73.823066
428.615273	77.049289	73.828071
427.635238	66.096579	73.833076
426.864599	70.322342	73.838081
426.354546	72.488219	73.843086
426.316311	67.738554	73.848090
425.372301	71.176714	73.853095
424.728422	71.736610	73.858100
423.931978	71.994410	73.863105
423.339990	69.045439	73.868110
422.156855	65.468470	73.873114
421.430206	64.649201	73.878119
421.346782	64.348714	73.883124
420.910553	67.961410	73.888129
420.380507	68.443248	73.893134
419.532213	67.274382	73.898138
418.789058	79.175012	73.903143
417.818692	72.150266	73.908148
416.545998	63.994218	73.913153
415.911018	68.371819	73.918158
415.785634	70.094805	73.923162
415.381626	76.622689	73.928167
415.441450	69.807498	73.933172
414.263602	74.331526	73.938177
412.896345	75.314181	73.943182
412.563981	63.174981	73.948186
412.146036	69.905343	73.953191
411.373532	69.705200	73.958196
410.383014	79.754611	73.963201
410.085849	68.459719	73.968206
409.876502	68.144607	73.973210
408.665275	74.075774	73.978215
408.019242	66.942585	73.983220
407.399107	79.665650	73.988225
406.839559	78.149596	73.993230
405.983451	74.179922	73.998234
405.228572	71.949148	74.003239
404.835532	59.445910	74.008244
404.347317	69.276509	74.013249
403.232141	65.162055	74.018254
402.750733	70.842891	74.023258
402.265027	80.576911	74.028263
401.903052	71.488894	74.033268
400.617834	56.690028	74.038273
399.963400	69.730766	74.043278
399.890925	67.632507	74.048282
398.451329	76.272824	74.053287
397.781872	69.009339	74.058292
397.172296	73.190521	74.063297
396.693675	72.219779	74.068302
396.396131	56.623324	74.073306
395.297473	76.822776	74.078311
395.013689	68.693640	74.083316
394.359362	75.460099	74.088321
393.736505	67.783940	74.093326
392.771600	71.227017	74.098330
391.671846	80.822365	74.103335
391.530661	70.824017	74.108340
391.259252	63.653212	74.113345
390.657001	70.321489	74.118350
389.435265	71.514340	74.123354
388.382767	69.863974	74.128359
388.530829	62.273110	74.133364
387.511398	64.690467	74.138369
386.528382	72.256730	74.143374
385.975557	64.381771	74.148378
385.414747	66.145763	74.153383
385.527435	64.144145	74.158388
384.328667	66.303097	74.163393
383.409958	66.321792	74.168398
382.894098	67.692295	74.173402
382.397659	66.718088	74.178407
381.611547	68.937427	74.183412
381.088699	64.905195	74.188417
380.432408	72.290091	74.193422
380.231766	60.087336	74.198426
378.816726	63.843409	74.203431
378.186326	62.784903	74.208436
377.783604	65.074022	74.213441
376.546119	68.155295	74.218446
376.144108	61.990835	74.223450
375.061554	70.347195	74.228455
375.064080	67.861695	74.233460
374.609003	68.260638	74.238465
374.181211	70.399223	74.243470
373.163074	66.099019	74.248474
372.193312	62.360348	74.253479
371.765907	70.076173	74.258484
370.544324	71.300544	74.263489
369.376083	71.716955	74.268494
369.353283	73.144492	74.273498
368.797310	66.455827	74.278503
368.586787	74.174934	74.283508
368.264387	71.723872	74.288513
367.406747	71.683957	74.293518
367.022946	62.583665	74.298522
366.109354	69.799848	74.303527
364.994739	62.862771	74.308532
364.285255	67.277485	74.313537
363.679322	73.555298	74.318542
363.348972	67.169698	74.323546
362.460154	71.344931	74.328551
361.638000	59.435184	74.333556
360.770574	76.748434	74.338561
360.417823	76.009934	74.343566
360.466121	59.551024	74.348570
358.907045	67.737344	74.353575
358.659674	62.396586	74.358580
357.967428	70.277614	74.363585
357.027589	66.901584	74.368590
356.527534	59.248446	74.373594
355.854967	70.554397	74.378599
355.592828	72.832154	74.383604
354.547810	72.560351	74.388609
353.517567	62.221193	74.393614
353.150440	57.452996	74.398618
352.944290	70.889041	74.403623
352.365099	62.568894	74.408628
351.029153	71.219518	74.413633
350.287769	67.475995	74.418638
350.147406	67.376960	74.423642
348.617712	66.914342	74.428647
348.209817	64.872698	74.433652
347.874160	61.665291	74.438657
347.246529	65.247005	74.443662
347.172351	55.930230	74.448666
345.940539	69.304251	74.453671
345.282988	65.323457	74.458676
345.002654	63.207871	74.463681
343.928102	69.667598	74.468686
343.286611	62.286146	74.473690
342.530921	74.132016	74.478695
341.984361	58.275662	74.483700
341.447758	72.863436	74.488705
340.477350	67.994282	74.493710
339.607476	64.614994	74.498714
338.787410	76.829071	74.503719
338.897380	66.580985	74.508724
338.504945	73.151182	74.513729
337.858429	63.580293	74.518734
336.969502	58.335484	74.523738
335.796224	71.753795	74.528743
334.887946	70.011086	74.533748
334.490523	71.853121	74.538753
333.940343	67.684917	74.543758
333.634773	58.318296	74.548762
333.024303	64.298810	74.553767
332.102991	71.260785	74.558772
331.138011	70.575716	74.563777
330.450945	62.212850	74.568782
330.302236	58.797468	74.573786
329.458337	69.067937	74.578791
328.723807	71.116656	74.583796
328.179135	82.015909	74.588801
327.274149	69.212684	74.593806
326.336917	64.677272	74.598810
325.224714	76.740809	74.603815
325.363354	74.711399	74.608820
324.960195	75.444251	74.613825
324.197102	75.288364	74.618830
324.129947	62.733205	74.623834
322.959407	88.166654	74.628839
322.492405	77.379784	74.633844
321.963250	75.877830	74.638849
320.683786	80.610472	74.643854
319.915158	69.193641	74.648858
319.082818	85.424332	74.653863
318.564114	71.799501	74.658868
318.393297	78.526754	74.663873
317.574624	80.215176	74.668878
317.077685	70.528993	74.673882
316.491295	83.197809	74.678887
315.667297	74.519322	74.683892
314.758864	73.222893	74.688897
314.271671	83.229953	74.693902
314.003623	66.290069	74.698906
313.007961	71.696517	74.703911
312.524731	70.789601	74.708916
312.093218	73.947430	74.713921
310.911577	83.145879	74.718926
310.340986	69.456789	74.723930
309.444411	78.541995	74.728935
308.978090	68.026245	74.733940
308.133049	71.620546	74.738945
307.289404	79.259234	74.743950
306.965863	66.462686	74.748954
306.737045	73.754230	74.753959
305.757178	81.143415	74.758964
305.011403	69.677219	74.763969
304.266672	77.547705	74.768974
304.004237	75.506535	74.773978
302.872147	76.161626	74.778983
302.181594	69.615847	74.783988
301.625341	76.082859	74.788993
301.008567	80.768224	74.793998
300.793841	79.023781	74.799002
299.389473	80.195327	74.804007
298.827887	72.619810	74.809012
298.721375	64.366253	74.814017
297.482268	68.562650	74.819022
296.909623	77.755486	74.824026
296.205123	69.018542	74.829031
295.831656	74.100332	74.834036
295.450167	77.806817	74.839041
294.357611	78.942856	74.844046
293.424663	63.351519	74.849050
292.918792	74.717638	74.854055
292.582680	68.724028	74.859060
292.125305	70.574048	74.864065
291.166186	82.360903	74.869070
290.455810	66.584286	74.874074
289.949272	83.898374	74.879079
288.965548	72.720831	74.884084
288.249316	73.215030	74.889089
287.679143	76.262511	74.894094
287.404105	74.917164	74.899098
286.701875	81.267110	74.904103
285.545595	72.061324	74.909108
284.851939	77.735013	74.914113
284.241452	74.241863	74.919118
284.323182	72.279867	74.924122
283.587974	83.116463	74.929127
282.452286	75.958871	74.934132
281.930698	75.534281	74.939137
281.239317	82.708766	74.944142
280.517213	78.635784	74.949146
279.612224	77.405046	74.954151
278.903187	73.224334	74.959156
278.791304	78.053132	74.964161
278.103262	81.423736	74.969166
277.359262	78.574723	74.974170
276.748721	78.905431	74.979175
276.201894	76.171635	74.984180
275.004434	76.617978	74.989185
274.269781	76.851784	74.994190
274.123590	70.947742	74.999194
273.380087	80.908936	75.004199
272.670188	69.476456	75.009204
272.023422	63.235927	75.014209
271.350751	75.344524	75.019214
271.197679	72.492773	75.024218
270.155453	71.462099	75.029223
269.429785	66.732148	75.034228
268.861548	74.347439	75.039233
267.503641	83.111988	75.044238
266.743076	67.330767	75.049242
266.074061	72.711968	75.054247
265.688957	75.876598	75.059252
265.563170	66.126538	75.064257
265.143527	79.814222	75.069262
264.218210	65.273439	75.074266
263.355761	83.379071	75.079271
263.000266	74.897140	75.084276
262.641567	66.351073	75.089281
261.118984	68.944875	75.094286
260.633145	71.048579	75.099290
260.373475	78.475923	75.104295
259.384336	67.231458	75.109300
258.688660	72.484456	75.114305
257.753637	83.786542	75.119310
257.643919	73.065734	75.124314
256.813801	72.989934	75.129319
256.037179	66.877334	75.134324
255.260401	67.155706	75.139329
254.534068	72.164450	75.144334
254.606298	75.961025	75.149338
253.621252	81.944507	75.154343
252.896958	76.500029	75.159348
252.733303	77.420200	75.164353
251.327127	79.645393	75.169358
250.744477	71.098761	75.174362
250.252325	75.448899	75.179367
249.508397	73.959124	75.184372
248.768579	79.775790	75.189377
247.952165	79.923297	75.194382
247.875151	72.535457	75.199386
247.139368	82.087023	75.204391
246.206957	68.652745	75.209396
245.227363	67.698824	75.214401
244.296893	82.082915	75.219406
244.507037	65.030553	75.224410
243.891736	75.263026	75.229415
242.859981	80.825056	75.234420
242.239944	72.424725	75.239425
241.120598	81.622730	75.244430
241.252899	74.310323	75.249434
240.149102	77.173244	75.254439
239.469883	82.234405	75.259444
238.933472	70.100969	75.264449
238.082917	79.038518	75.269454
237.710485	69.274168	75.274458
236.595785	88.701999	75.279463
236.006408	80.612146	75.284468
235.830684	81.408095	75.289473
235.443782	83.742020	75.294478
234.713461	76.516675	75.299482
233.861755	76.174684	75.304487
233.246851	87.108800	75.309492
232.117020	79.112994	75.314497
231.284419	78.126183	75.319502
230.983635	72.939026	75.324506
230.556717	80.601178	75.329511
229.991817	78.494705	75.334516
229.021165	69.093792	75.339521
228.102959	76.130993	75.344526
228.000058	67.414853	75.349530
227.319577	69.563785	75.354535
226.323237	75.755640	75.359540
225.950352	72.875864	75.364545
225.226207	76.042515	75.369550
223.932573	72.927934	75.374554
223.503500	81.430888	75.379559
223.031778	74.648412	75.384564
222.874213	81.148064	75.389569
221.984171	89.833316	75.394574
220.906177	74.744492	75.399578
220.282620	76.753474	75.404583
219.909789	75.046861	75.409588
219.437190	62.236260	75.414593
217.896827	76.544134	75.419598
217.545488	79.162530	75.424602
217.177504	77.499296	75.429607
216.598396	78.569277	75.434612
216.211626	73.411600	75.439617
214.867995	82.262199	75.444622
214.602045	78.441344	75.449626
214.218237	77.411371	75.454631
213.119951	87.019164	75.459636
212.554196	70.341220	75.464641
211.471972	80.217666	75.469646
211.303348	75.222315	75.474650
210.186965	66.804944	75.479655
209.204290	72.155746	75.484660
208.991264	76.667955	75.489665
208.395587	70.936503	75.494670
208.369981	64.363587	75.499674
207.767980	71.905428	75.504679
207.205849	76.815471	75.509684
206.406076	68.120558	75.514689
204.695246	81.586780	75.519694
203.960450	70.338059	75.524698
203.624637	66.697069	75.529703
203.043487	66.034429	75.534708
203.319993	72.483793	75.539713
201.949152	73.593282	75.544718
200.939601	66.904448	75.549722
200.205901	78.611232	75.554727
200.095868	70.902257	75.559732
199.935231	75.953278	75.564737
198.820906	81.771323	75.569742
198.189112	77.981993	75.574746
197.348502	77.163616	75.579751
196.547257	86.768207	75.584756
195.890665	81.237264	75.589761
195.223122	70.179660	75.594766
194.947343	69.022088	75.599770
193.914793	76.367669	75.604775
192.900589	76.822677	75.609780
192.356687	80.018943	75.614785
191.746657	85.088006	75.619790
191.829310	81.642051	75.624794
191.195120	79.075159	75.629799
189.974553	73.914819	75.634804
189.427654	74.295322	75.639809
188.862780	81.020753	75.644814
188.218856	63.727707	75.649818
187.210933	80.543033	75.654823
186.577535	79.267450	75.659828
186.619604	72.171269	75.664833
185.318992	75.287928	75.669838
184.864941	73.893871	75.674842
184.002647	81.480376	75.679847
183.568106	70.196404	75.684852
183.064877	69.585995	75.689857
181.962157	78.929591	75.694862
181.808286	78.676612	75.699866
181.277904	71.288533	75.704871
179.793772	73.578230	75.709876
179.434386	71.336508	75.714881
178.602891	77.782775	75.719886
178.548680	80.150387	75.724890
177.576419	81.139572	75.729895
176.506184	73.284098	75.734900
176.334167	77.185840	75.739905
175.651267	76.030109	75.744910
175.167900	79.781236	75.749914
173.983832	80.988684	75.754919
173.292893	80.972717	75.759924
173.131510	77.370145	75.764929
171.989271	86.502446	75.769934
171.103175	78.668071	75.774938
170.686627	80.738668	75.779943
169.991155	71.642388	75.784948
169.866069	79.409371	75.789953
169.112194	88.765159	75.794958
168.560467	76.930632	75.799962
167.790045	79.420328	75.804967
167.113738	73.258651	75.809972
166.165384	61.498417	75.814977
165.027492	81.339931	75.819982
164.685288	81.389777	75.824986
164.476972	83.788270	75.829991
164.029860	75.675759	75.834996
162.987904	70.606797	75.840001
162.291517	76.474899	75.845006
161.842759	72.098194	75.850010
161.291216	80.920281	75.855015
159.937494	78.873378	75.860020
159.781483	69.615396	75.865025
159.069614	78.078296	75.870030
158.588426	82.305285	75.875034
157.462319	84.388108	75.880039
156.911384	83.715930	75.885044
156.752388	72.842159	75.890049
155.662943	83.293747	75.895054
154.737789	74.598346	75.900058
154.115953	74.473601	75.905063
153.614506	83.620415	75.910068
153.448008	71.833273	75.915073
152.665186	82.185509	75.920078
151.738911	76.450021	75.925082
151.351940	69.433295	75.930087
150.500221	78.528735	75.935092
149.522530	77.000578	75.940097
148.812439	82.853526	75.945102
148.476800	75.478553	75.950106
147.845667	73.511964	75.955111
147.019078	77.738840	75.960116
146.337238	73.981160	75.965121
145.496391	81.397110	75.970126
144.981496	75.339002	75.975130
144.595043	84.767082	75.980135
144.156868	75.505210	75.985140
143.708757	77.612381	75.990145
142.673157	80.358820	75.995150
141.901633	76.147119	76.000154
140.917273	78.677245	76.005159
140.648290	85.823825	76.010164
140.253891	75.369189	76.015169
139.021262	83.058911	76.020174
138.510003	76.446753	76.025178
138.102975	85.135422	76.030183
137.359726	78.664328	76.035188
136.156307	76.538282	76.040193
134.961214	83.925575	76.045198
134.797758	78.623501	76.050202
134.447623	76.066519	76.055207
134.163948	89.522813	76.060212
134.068071	81.338531	76.065217
132.821654	82.981688	76.070222
132.387429	73.936796	76.075226
131.430905	78.624336	76.080231
130.374389	80.038530	76.085236
129.956431	74.614628	76.090241
129.308669	88.151055	76.095246
129.001897	83.795864	76.100250
127.926481	88.078197	76.105255
127.216150	87.100307	76.110260
126.968537	77.880586	76.115265
126.105359	81.236580	76.120270
125.118678	87.463202	76.125274
124.538559	78.392692	76.130279
124.020393	78.645633	76.135284
123.528648	72.036677	76.140289
122.290521	80.925682	76.145294
121.587400	86.266629	76.150298
121.621082	85.707798	76.155303
120.825369	87.624417	76.160308
120.359657	72.300833	76.165313
119.509045	75.107660	76.170318
118.623885	72.536660	76.175322
118.248400	82.659955	76.180327
117.405641	84.645574	76.185332
116.661128	77.812017	76.190337
116.307553	81.769520	76.195342
115.602240	79.425289	76.200346
114.638123	77.379355	76.205351
113.553677	75.868238	76.210356
113.479567	81.403745	76.215361
112.774199	87.763693	76.220366
112.394240	81.352936	76.225370
111.455281	67.017822	76.230375
110.538850	78.745878	76.235380
110.331232	71.618562	76.240385
109.498580	81.704383	76.245390
108.992360	76.229910	76.250394
108.183383	76.250130	76.255399
107.680663	75.306943	76.260404
106.951917	76.604225	76.265409
105.681014	76.433202	76.270414
105.141601	69.688361	76.275418
104.677299	73.192046	76.280423
104.248560	80.543862	76.285428
103.986762	73.231236	76.290433
102.636480	86.520180	76.295438
102.613770	71.911221	76.300442
101.916440	77.235478	76.305447
100.493046	71.144085	76.310452
100.183741	74.414910	76.315457
99.306605	70.937532	76.320462
99.012587	76.840821	76.325466
98.322819	84.245305	76.330471
96.741123	85.943527	76.335476
96.231151	72.719479	76.340481
95.789124	76.910271	76.345486
95.320144	78.956127	76.350490
95.102654	80.682775	76.355495
94.608701	83.726024	76.360500
94.679157	83.932404	76.365505
93.740737	75.116153	76.370510
92.880682	81.439275	76.375514
91.995723	78.836716	76.380519
90.796910	76.503393	76.385524
89.828772	74.685176	76.390529
88.721415	78.725052	76.395534
88.396637	76.007927	76.400538
88.668068	72.582326	76.405543
87.883729	72.305332	76.410548
87.761656	67.023474	76.415553
86.564083	76.379076	76.420558
85.956812	85.377207	76.425562
85.332148	75.293600	76.430567
83.748418	83.994907	76.435572
83.242210	77.426110	76.440577
82.792586	79.684908	76.445582
82.573826	82.140261	76.450586
82.311682	74.190649	76.455591
81.341759	80.083473	76.460596
80.447765	70.413383	76.465601
79.767517	85.645368	76.470606
79.231985	67.042070	76.475610
78.508476	64.327044	76.480615
77.328230	81.940954	76.485620
77.480663	72.127626	76.490625
76.486958	76.042155	76.495630
75.389747	68.564751	76.500634
74.767329	67.435672	76.505639
74.365309	70.060589	76.510644
73.930255	66.252537	76.515649
73.627829	72.702753	76.520654
72.684567	71.451393	76.525658
72.171374	76.758902	76.530663
70.991681	75.201499	76.535668
70.105519	62.367028	76.540673
69.530695	75.117590	76.545678
69.123238	73.725586	76.550682
68.866674	81.920361	76.555687
68.022065	76.138772	76.560692
67.214252	61.273452	76.565697
66.509767	80.178603	76.570702
66.049136	79.555117	76.575706
65.447519	80.128864	76.580711
64.001854	75.233138	76.585716
64.086484	67.445830	76.590721
63.330099	72.923005	76.595726
62.772103	73.727898	76.600730
61.740574	78.638722	76.605735
60.855794	85.907172	76.610740
60.994402	73.685058	76.615745
60.334823	82.306785	76.620750
59.393128	76.371962	76.625754
58.716890	80.781452	76.630759
57.877668	82.897404	76.635764
57.051512	71.365293	76.640769
56.185544	73.506009	76.645774
55.206989	80.492969	76.650778
54.919188	75.896665	76.655783
54.345308	82.405950	76.660788
54.388309	77.523511	76.665793
54.138589	77.847183	76.670798
53.085169	85.336485	76.675802
52.646614	72.208287	76.680807
51.319998	84.813858	76.685812
50.494255	80.085750	76.690817
49.922816	81.696979	76.695822
49.421111	80.782025	76.700826
48.798134	77.005526	76.705831
47.501651	89.437574	76.710836
47.462260	82.936244	76.715841
46.838878	78.559033	76.720846
46.538922	86.270335	76.725850
45.695546	84.977823	76.730855
44.441355	81.256274	76.735860
44.369779	74.414753	76.740865
43.344048	76.899478	76.745870
42.321519	75.772729	76.750874
41.884436	81.339322	76.755879
41.251545	79.134939	76.760884
41.091508	76.197594	76.765889
40.153827	81.579124	76.770894
39.496648	89.178683	76.775898
39.004539	79.923865	76.780903
38.184561	81.308253	76.785908
37.671348	83.168800	76.790913
36.750845	82.200809	76.795918
36.286938	78.107225	76.800922
35.839349	72.615537	76.805927
34.641398	79.577578	76.810932
33.846053	71.916437	76.815937
33.334149	80.410542	76.820942
33.170259	77.189981	76.825946
32.743545	69.547308	76.830951
31.290562	75.059914	76.835956
30.971117	71.843667	76.840961
30.259172	82.701827	76.845966
29.228722	77.774584	76.850970
28.704158	74.789736	76.855975
27.949114	76.089659	76.860980
28.155864	74.730570	76.865985
26.993084	82.519577	76.870990
26.001468	80.165852	76.875994
25.855528	65.718485	76.880999
25.136417	80.111483	76.886004
24.392747	75.256762	76.891009
23.530374	71.050137	76.896014
22.776878	76.186264	76.901018
22.713076	75.997771	76.906023
21.437378	75.739254	76.911028
20.722013	64.853343	76.916033
20.354137	82.277769	76.921038
19.812926	82.476065	76.926042
19.121376	67.432956	76.931047
17.865444	77.784995	76.936052
17.929173	69.710883	76.941057
17.120893	67.074049	76.946062
16.242359	72.698443	76.951066
15.396790	79.933843	76.956071
14.694617	78.568361	76.961076
14.423132	76.391487	76.966081
13.842789	69.639010	76.971086
13.299690	86.239898	76.976090
12.307484	87.393166	76.981095
11.721117	78.736823	76.986100
11.453592	74.250825	76.991105
10.610985	79.500512	76.996110
9.513868	73.950025	77.001114
8.997916	72.766136	77.006119
8.283273	86.663303	77.011124
7.773564	82.163899	77.016129
6.931577	81.601257	77.021134
6.396581	76.150324	77.026139
6.339395	78.221964	77.031143
5.127158	87.600442	77.036148
4.305871	74.109140	77.041153
3.937785	75.963888	77.046158