Tue Jun 21 10:25:02 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
1.534763	109.969481	0.000000
1.189202	99.697457	0.005005
1.039047	98.994042	0.010010
1.214788	92.565437	0.015014
0.951499	97.656171	0.020019
0.977463	85.015192	0.025024
0.616762	71.601749	0.030029
0.467658	59.544095	0.035034
0.097359	56.034132	0.040038
-0.109460	53.015299	0.045043
-0.794586	36.545415	0.050048
-0.930408	30.128765	0.055053
-1.145407	26.864031	0.060058
-1.172768	12.128948	0.065062
-1.813577	17.327755	0.070067
-2.143645	15.275755	0.075072
-2.211537	11.546018	0.080077
-2.870144	9.954142	0.085082
-2.624729	3.563371	0.090086
-3.038650	2.150808	0.095091
-3.818986	-1.736034	0.100096
-3.918613	-0.744226	0.105101
-4.622292	0.838182	0.110106
-4.478851	4.938207	0.115110
-4.573739	6.270027	0.120115
-4.730103	3.939834	0.125120
-4.715045	3.821787	0.130125
-4.894510	9.131466	0.135130
-5.260171	1.811801	0.140134
-6.194220	4.101518	0.145139
-6.322143	3.485594	0.150144
-6.464438	4.323444	0.155149
-6.710705	0.601540	0.160154
-6.583187	-5.257622	0.165158
-6.673338	-2.300555	0.170163
-7.204581	-2.748853	0.175168
-7.663793	4.314090	0.180173
-7.892014	0.135132	0.185178
-8.259823	2.161375	0.190182
-8.201483	0.308106	0.195187
-8.733152	-3.328844	0.200192
-9.046259	0.782648	0.205197
-9.342806	4.126334	0.210202
-9.171273	-8.102565	0.215206
-9.491108	7.642694	0.220211
-9.426571	-10.159753	0.225216
-9.855054	-0.683770	0.230221
-10.707855	-1.293124	0.235226
-10.660140	-9.770521	0.240230
-11.066620	1.733572	0.245235
-11.404796	0.312808	0.250240
-11.143377	5.497183	0.255245
-11.233651	4.165016	0.260250
-11.356893	-2.258636	0.265254
-12.279756	8.573999	0.270259
-12.570229	-2.557192	0.275264
-12.750947	1.142050	0.280269
-12.933653	4.015187	0.285274
-12.742333	-6.198853	0.290278
-13.168332	4.967481	0.295283
-13.663060	4.105050	0.300288
-14.167322	5.690352	0.305293
-14.702992	-2.096465	0.310298
-14.492712	3.760407	0.315302
-14.627799	-0.872252	0.320307
-14.461547	4.813916	0.325312
-14.397339	3.825972	0.330317
-15.346929	-5.302253	0.335322
-15.642404	-1.007003	0.340326
-16.321005	9.212915	0.345331
-16.188495	6.978742	0.350336
-16.384740	-1.631321	0.355341
-16.349904	2.843269	0.360346
-16.277940	-0.616188	0.365350
-17.293373	1.712859	0.370355
-17.515798	3.011334	0.375360
-17.664552	2.450562	0.380365
-17.804945	3.460763	0.385370
-17.536460	-6.076963	0.390374
-18.508583	-0.877563	0.395379
-19.266057	-5.855891	0.400384
-19.291856	-6.472150	0.405389
-19.326079	-0.562753	0.410394
-19.446406	-1.954076	0.415398
-19.732838	5.450454	0.420403
-19.561014	0.284292	0.425408
-19.810777	3.650818	0.430413
-20.216943	6.071965	0.435418
-20.524939	0.070024	0.440422
-20.979272	3.796028	0.445427
-21.123482	-1.886121	0.450432
-20.969621	2.243553	0.455437
-21.350474	3.435458	0.460442
-21.998760	-1.684484	0.465446
-22.200400	-0.348208	0.470451
-22.050122	-5.831073	0.475456
-22.289510	-0.260269	0.480461
-23.042114	5.487484	0.485466
-23.089193	6.556036	0.490470
-23.614474	-1.088051	0.495475
-23.434873	-1.883760	0.500480
-23.338140	-1.277104	0.505485
-24.098690	-0.921574	0.510490
-24.614536	0.821147	0.515494
-25.083037	-3.089702	0.520499
-25.583788	2.826504	0.525504
-25.076379	0.692654	0.530509
-25.322450	4.396011	0.535514
-25.105843	-1.912435	0.540518
-25.657393	9.454858	0.545523
-25.735710	-2.142639	0.550528
-26.596330	5.535169	0.555533
-26.630306	6.431449	0.560538
-26.752741	3.442858	0.565542
-27.394957	-1.402610	0.570547
-26.910434	-2.946784	0.575552
-27.584330	-5.869903	0.580557
-28.230153	5.315074	0.585562
-28.122733	-5.474903	0.590566
-28.257228	2.291634	0.595571
-28.247030	-1.185814	0.600576
-28.543429	-2.497462	0.605581
-29.892051	11.044040	0.610586
-29.858893	-4.342381	0.615590
-30.063673	8.165502	0.620595
-29.928663	-7.791897	0.625600
-29.913608	-0.549382	0.630605
-30.600761	-6.725529	0.635610
-30.132514	-1.061748	0.640614
-30.467484	-3.122600	0.645619
-31.225396	-0.158748	0.650624
-31.534219	-1.835182	0.655629
-31.735277	8.714136	0.660634
-31.603977	-3.543425	0.665638
-31.762482	-2.432149	0.670643
-32.477756	-2.625796	0.675648
-32.858812	-0.926314	0.680653
-33.380886	-3.945417	0.685658
-33.260889	0.600120	0.690662
-33.519132	6.125506	0.695667
-33.515929	0.288310	0.700672
-33.403041	-1.674435	0.705677
-34.068087	1.072363	0.710682
-34.578920	-8.732946	0.715686
-34.700118	-9.426943	0.720691
-34.867591	-2.082372	0.725696
-34.942636	0.726759	0.730701
-35.150043	-2.454171	0.735706
-35.575965	0.517653	0.740710
-36.347354	6.659437	0.745715
-36.180279	3.865623	0.750720
-36.334103	-4.988064	0.755725
-36.757253	3.387690	0.760730
-36.493498	-5.266577	0.765734
-36.847538	3.186928	0.770739
-37.420961	0.717813	0.775744
-37.725181	-0.717451	0.780749
-37.962304	-3.186610	0.785754
-37.932243	0.676245	0.790758
-38.077555	-6.513548	0.795763
-38.819384	1.890905	0.800768
-39.192398	-7.933872	0.805773
-39.641892	-1.386201	0.810778
-39.638173	2.073324	0.815782
-39.866768	-3.553013	0.820787
-39.532508	-4.653759	0.825792
-39.827885	5.475068	0.830797
-40.575345	5.464747	0.835802
-40.880918	-11.029053	0.840806
-41.600238	2.323769	0.845811
-41.419924	-6.138092	0.850816
-41.474943	-0.710102	0.855821
-41.421448	-8.197442	0.860826
-41.789288	-3.136787	0.865830
-41.724452	-0.610315	0.870835
-42.375553	-0.387360	0.875840
-42.879764	-3.869603	0.880845
-43.049718	-1.873163	0.885850
-43.332485	-15.640815	0.890854
-43.488839	-4.333254	0.895859
-43.241888	-10.097540	0.900864
-43.285863	-9.725106	0.905869
-44.342626	1.716573	0.910874
-44.526715	-5.902906	0.915878
-44.998519	-1.526556	0.920883
-44.801904	-4.936995	0.925888
-44.556097	-2.252829	0.930893
-45.930529	5.632615	0.935898
-45.897412	-5.215898	0.940902
-46.072818	-4.232655	0.945907
-46.226919	-3.213079	0.950912
-46.016626	1.604230	0.955917
-46.393000	0.093892	0.960922
-46.862743	-12.242515	0.965926
-47.279202	-2.926392	0.970931
-47.530466	-3.944578	0.975936
-47.615392	-1.673125	0.980941
-48.026574	-0.829423	0.985946
-47.725896	-0.023886	0.990950
-48.577141	0.495656	0.995955
-48.605478	-8.265145	1.000960
-48.704403	-5.097846	1.005965
-49.267059	2.573243	1.010970
-49.053572	-4.332410	1.015974
-49.361561	2.054485	1.020979
-50.269295	-7.325945	1.025984
-50.969239	-4.715447	1.030989
-51.166735	0.471315	1.035994
-50.861238	0.685630	1.040998
-51.087781	-6.586416	1.046003
-51.101949	-5.460562	1.051008
-50.981810	-7.866733	1.056013
-51.474597	0.014588	1.061018
-51.385808	-7.203908	1.066022
-52.192580	6.104398	1.071027
-52.420241	2.928795	1.076032
-52.530710	-6.804483	1.081037
-52.824479	5.561450	1.086042
-53.376535	-4.886852	1.091046
-53.787225	0.511238	1.096051
-53.937260	-2.061142	1.101056
-54.272559	10.044087	1.106061
-54.232044	-1.137175	1.111066
-54.198470	-7.400507	1.116070
-54.112372	7.214287	1.121075
-54.807351	-5.511657	1.126080
-55.487907	2.784971	1.131085
-55.886247	4.513958	1.136090
-55.842131	-4.925635	1.141094
-55.999437	9.601400	1.146099
-55.930167	7.639562	1.151104
-55.747298	-3.916527	1.156109
-56.899273	5.693878	1.161114
-57.264082	-1.625523	1.166118
-57.878725	6.155015	1.171123
-57.755456	3.957498	1.176128
-57.795920	-3.381871	1.181133
-57.829595	7.304893	1.186138
-57.616077	5.455919	1.191142
-58.157029	2.361406	1.196147
-58.689652	9.365864	1.201152
-59.098175	9.738682	1.206157
-59.386468	9.665347	1.211162
-58.760954	5.510571	1.216166
-59.382905	8.695818	1.221171
-60.437052	8.325243	1.226176
-60.662744	1.383391	1.231181
-60.941757	5.007350	1.236186
-60.945555	-2.218705	1.241190
-60.867042	-0.752407	1.246195
-61.100124	-3.695439	1.251200
-60.747659	-8.286487	1.256205
-61.769091	10.409859	1.261210
-62.204179	-0.142471	1.266214
-62.487240	4.500599	1.271219
-62.779038	-6.250690	1.276224
-62.361190	0.139728	1.281229
-62.628315	6.870914	1.286234
-62.775501	-5.764001	1.291238
-63.864913	-0.179311	1.296243
-63.909440	-0.560600	1.301248
-63.982164	-1.727543	1.306253
-64.397750	13.685477	1.311258
-64.337545	8.178255	1.316262
-64.153280	5.051256	1.321267
-65.300583	7.988236	1.326272
-65.333371	2.297109	1.331277
-65.922993	12.040336	1.336282
-65.525145	1.854252	1.341286
-65.689417	9.832134	1.346291
-65.971075	9.958587	1.351296
-66.063926	0.739206	1.356301
-66.931781	5.129251	1.361306
-67.001670	-1.931543	1.366310
-67.350145	-2.613948	1.371315
-67.432559	4.504601	1.376320
-67.280887	6.927300	1.381325
-68.339322	6.089755	1.386330
-68.669418	-2.440709	1.391334
-68.772255	2.830623	1.396339
-68.948219	7.095034	1.401344
-68.833048	4.999301	1.406349
-69.220581	7.675874	1.411354
-68.683619	-5.040374	1.416358
-69.833936	1.228892	1.421363
-70.275730	6.468349	1.426368
-70.445812	2.462697	1.431373
-70.594898	16.068798	1.436378
-70.560873	-0.638324	1.441382
-70.808590	5.656894	1.446387
-71.121703	0.352200	1.451392
-71.570570	0.956661	1.456397
-71.999733	6.418197	1.461402
-71.994219	5.396362	1.466406
-72.306472	1.990274	1.471411
-72.082410	0.613551	1.476416
-72.180845	-6.858493	1.481421
-73.086478	4.434434	1.486426
-73.238794	-3.772440	1.491430
-73.793000	5.774096	1.496435
-73.647958	4.638183	1.501440
-73.622932	3.963582	1.506445
-74.477812	1.390124	1.511450
-74.667893	-8.456851	1.516454
-74.781121	8.567444	1.521459
-75.039025	5.035335	1.526464
-74.754349	0.743421	1.531469
-75.192353	0.898727	1.536474
-75.666390	1.269372	1.541478
-76.322874	0.728949	1.546483
-76.526292	-2.501182	1.551488
-76.416905	1.279072	1.556493
-76.976278	3.473798	1.561498
-76.671755	-2.903079	1.566502
-77.049373	0.453837	1.571507
-77.705203	0.849854	1.576512
-77.890941	-2.934952	1.581517
-78.321716	-1.564673	1.586522
-78.213244	-1.198541	1.591526
-78.484906	-0.510946	1.596531
-78.345179	6.880629	1.601536
-78.830950	-1.987937	1.606541
-79.853087	3.385520	1.611546
-79.556379	-7.472701	1.616550
-79.874588	5.044883	1.621555
-80.045130	-3.687630	1.626560
-79.857858	-1.958735	1.631565
-80.324906	10.232642	1.636570
-80.700818	5.258622	1.641574
-81.426916	5.141762	1.646579
-81.502048	1.397838	1.651584
-81.576382	-0.677955	1.656589
-81.895487	7.604005	1.661594
-81.741245	1.795868	1.666598
-82.052468	6.132999	1.671603
-82.539255	4.259305	1.676608
-83.026003	-4.549501	1.681613
-83.339245	4.449585	1.686618
-83.574636	-3.424046	1.691622
-83.233686	1.522779	1.696627
-83.359521	3.908555	1.701632
-83.508612	0.906622	1.706637
-84.426504	10.391835	1.711642
-84.534298	-1.601164	1.716646
-84.841610	8.334279	1.721651
-85.066439	4.452346	1.726656
-85.090034	4.830878	1.731661
-85.707469	3.397960	1.736666
-86.025047	4.740612	1.741670
-86.006826	7.336175	1.746675
-86.226642	-3.497679	1.751680
-86.234811	-3.140250	1.756685
-86.846960	1.818394	1.761690
-86.702703	-5.821912	1.766694
-87.205107	2.871060	1.771699
-87.752425	-1.149272	1.776704
-87.680364	6.076302	1.781709
-88.012312	-2.149958	1.786714
-87.826517	1.322035	1.791718
-88.848159	2.347353	1.796723
-89.348007	5.898169	1.801728
-89.581872	2.761683	1.806733
-89.779744	6.186711	1.811738
-89.671133	6.332003	1.816742
-89.851235	2.503640	1.821747
-89.786608	0.999795	1.826752
-89.629722	-0.508871	1.831757
-90.226223	0.591473	1.836762
-90.481657	-0.090749	1.841766
-90.991146	0.162238	1.846771
-91.181808	0.981065	1.851776
-91.274251	-8.993966	1.856781
-92.079859	8.590179	1.861786
-92.524488	1.579214	1.866790
-92.794606	2.200250	1.871795
-92.859351	0.957000	1.876800
-92.799914	-4.679145	1.881805
-92.978051	6.112446	1.886810
-92.810533	-0.794672	1.891814
-92.946369	-1.157286	1.896819
-93.759774	7.622123	1.901824
-94.240767	-5.539047	1.906829
-94.262789	-4.182196	1.911834
-94.074996	-9.184054	1.916838
-94.739712	-6.099862	1.921843
-95.068784	-11.466434	1.926848
-95.664182	-6.091824	1.931853
-95.988040	0.155421	1.936858
-96.006969	-5.572924	1.941862
-95.888727	1.244607	1.946867
-96.626602	-0.281435	1.951872
-96.636557	-7.292358	1.956877
-96.934277	1.735335	1.961882
-96.398868	-6.040003	1.966886
-97.001560	-2.081040	1.971891
-97.695929	-1.868276	1.976896
-97.472863	-8.184695	1.981901
-97.774045	6.090879	1.986906
-98.300648	-2.877676	1.991910
-98.847608	-10.104936	1.996915
-99.155024	-3.500298	2.006912
-98.232153	3.298917	2.016909
-98.352257	0.591293	2.026906
-97.692546	6.118166	2.036902
-96.718754	-2.413108	2.046899
-96.639016	-0.939502	2.056896
-96.161779	-0.440628	2.066893
-95.349701	3.549670	2.076890
-95.198587	4.327212	2.086886
-94.423763	6.481580	2.096883
-93.818311	7.607305	2.106880
-93.653689	-3.431691	2.116877
-93.081208	2.336260	2.126874
-92.132343	2.789430	2.136870
-91.988367	-0.826371	2.146867
-92.089512	2.003591	2.156864
-90.913147	0.941333	2.166861
-90.867370	-2.172734	2.176858
-90.093149	5.087177	2.186854
-89.149292	0.342078	2.196851
-89.211117	1.402857	2.206848
-88.123217	-0.268530	2.216845
-87.723431	2.635355	2.226842
-87.739489	3.532461	2.236838
-87.413747	-6.284667	2.246835
-86.436718	7.433169	2.256832
-85.994774	2.195427	2.266829
-85.097786	9.726252	2.276826
-84.654290	5.826111	2.286822
-84.835876	4.335923	2.296819
-84.393202	1.203150	2.306816
-83.756752	4.581171	2.316813
-82.809642	-0.555687	2.326810
-82.000986	3.591077	2.336806
-81.776667	-1.474091	2.346803
-81.756217	1.279026	2.356800
-81.196838	1.495185	2.366797
-80.408408	3.949215	2.376794
-80.157105	6.047037	2.386790
-79.151839	-5.500074	2.396787
-78.643286	1.594987	2.406784
-78.399829	0.849847	2.416781
-78.489006	-5.177415	2.426778
-77.335648	-1.987746	2.436774
-76.738618	-0.981349	2.446771
-76.619597	0.401974	2.456768
-75.733400	-2.868862	2.466765
-75.538056	2.669321	2.476762
-75.495114	1.932493	2.486758
-74.328694	1.538544	2.496755
-73.863227	-1.175168	2.506752
-73.482340	-1.456411	2.516749
-72.664115	-0.691148	2.526746
-72.359505	3.455909	2.536742
-72.263068	0.144361	2.546739
-71.669522	0.050579	2.556736
-70.941742	0.292990	2.566733
-70.600158	0.793389	2.576730
-69.578936	-3.453163	2.586726
-68.934614	-2.789705	2.596723
-68.923927	-1.257835	2.606720
-68.799656	0.347694	2.616717
-68.063437	3.357096	2.626714
-67.742726	5.382567	2.636710
-66.451676	6.346149	2.646707
-65.776234	0.556605	2.656704
-66.031774	1.856734	2.666701
-65.837295	-2.008289	2.676698
-64.943203	7.347536	2.686694
-64.350724	4.743592	2.696691
-64.323446	1.800338	2.706688
-63.085123	2.768898	2.716685
-63.034922	0.329449	2.726682
-62.699801	-1.846777	2.736678
-61.617282	-1.676548	2.746675
-61.187245	-0.627872	2.756672
-61.331017	-6.435664	2.766669
-60.700658	0.215601	2.776666
-60.044342	1.815414	2.786662
-58.815482	-1.408828	2.796659
-58.819124	0.532048	2.806656
-58.519625	-3.076116	2.816653
-58.179287	-5.615777	2.826650
-57.328150	4.016671	2.836646
-56.588859	-2.677920	2.846643
-56.371411	4.639232	2.856640
-56.120710	-2.709270	2.866637
-55.253934	5.986794	2.876634
-55.009254	3.280404	2.886630
-54.587077	-0.076000	2.896627
-53.694007	-0.292884	2.906624
-53.402484	-0.932963	2.916621
-53.022974	-2.582857	2.926618
-51.994608	-2.760104	2.936614
-51.786291	0.620458	2.946611
-51.649258	-6.519930	2.956608
-51.105353	-3.851524	2.966605
-50.461794	-5.931033	2.976602
-49.955067	-5.550847	2.986598
-49.013188	-7.445025	2.996595
-48.814552	-2.685088	3.006592
-48.766795	6.272475	3.016589
-47.802594	4.684217	3.026586
-47.259919	3.949594	3.036582
-47.113362	-0.317684	3.046579
-46.242787	-0.351037	3.056576
-45.515906	-1.945240	3.066573
-45.451742	3.778272	3.076570
-45.303962	7.431652	3.086566
-44.146981	4.830846	3.096563
-44.145424	3.059787	3.106560
-43.190232	4.428724	3.116557
-42.547878	7.262609	3.126554
-42.321388	2.508873	3.136550
-42.163820	9.116334	3.146547
-41.316073	-1.302748	3.156544
-40.932724	1.363401	3.166541
-40.702789	2.285171	3.176538
-39.323003	-3.704589	3.186534
-39.023408	-1.320752	3.196531
-38.843632	-4.328382	3.206528
-38.780738	-7.568776	3.216525
-38.120676	4.182428	3.226522
-37.594838	-3.834233	3.236518
-36.315879	-2.148041	3.246515
-36.220305	1.003024	3.256512
-36.097610	3.430185	3.266509
-35.513785	1.914603	3.276506
-34.774724	0.837248	3.286502
-34.515196	8.515342	3.296499
-33.419144	4.950526	3.306496
-32.965118	10.447656	3.316493
-33.557157	10.030758	3.326490
-32.322043	7.708655	3.336486
-31.478298	5.668313	3.346483
-31.503982	2.400302	3.356480
-31.052254	3.055748	3.366477
-30.093636	0.786350	3.376474
-29.857774	-3.084736	3.386470
-29.598352	4.605230	3.396467
-28.725220	6.119550	3.406464
-28.487171	7.588282	3.416461
-27.749120	6.322794	3.426458
-26.779566	5.133966	3.436454
-26.455175	4.264184	3.446451
-26.281488	-2.314412	3.456448
-26.287343	1.216220	3.466445
-25.768516	-3.811767	3.476442
-25.285820	1.370402	3.486438
-23.770529	3.482779	3.496435
-23.557070	3.772630	3.506432
-23.403669	0.859664	3.516429
-23.219010	7.459281	3.526426
-22.269790	4.757144	3.536422
-22.139333	1.044392	3.546419
-20.825295	1.982249	3.556416
-20.524246	4.934699	3.566413
-20.398736	2.954616	3.576410
-20.281836	-1.040811	3.586406
-19.083760	-1.569801	3.596403
-19.005699	-3.107534	3.606400
-18.266013	0.101063	3.616397
-17.470201	1.741802	3.626394
-17.258732	2.014793	3.636390
-16.791166	5.164523	3.646387
-16.592947	1.322195	3.656384
-15.543698	-0.365892	3.666381
-15.411937	4.528024	3.676378
-14.975120	1.407290	3.686374
-14.309421	3.636452	3.696371
-13.857377	2.921385	3.706368
-12.815026	5.621660	3.716365
-12.512264	-0.246647	3.726362
-12.539275	6.340602	3.736358
-12.152922	4.552451	3.746355
-11.201876	5.744452	3.756352
-10.703343	3.014994	3.766349
-10.436147	-0.710126	3.776346
-9.410568	1.319748	3.786342
-8.996288	6.413667	3.796339
-8.796735	0.083895	3.806336
-8.682400	3.831729	3.816333
-7.731661	1.191979	3.826330
-7.356137	6.534360	3.836326
-6.749903	5.341286	3.846323
-5.863357	4.970386	3.856320
-5.765692	4.660769	3.866317
-5.677985	4.857437	3.876314
-4.958726	13.469078	3.886310
-4.388531	9.213644	3.896307
-3.928937	23.534296	3.906304
-3.383034	21.163911	3.916301
-2.959852	32.178645	3.926298
-2.675794	43.139959	3.936294
-1.875495	47.705245	3.946291
-1.703589	55.878410	3.956288
-1.165413	65.705199	3.966285
-0.852560	88.318467	3.976282
-0.626864	103.756361	3.986278
0.000000	117.102827	3.991283
0.105294	124.279547	3.996288
0.553822	135.944671	4.001293
0.714644	140.278657	4.006298
1.006454	146.969840	4.011302
1.229521	144.522724	4.016307
1.115457	166.905411	4.021312
1.277158	152.305833	4.026317
0.971322	135.932285	4.031322
0.868710	138.082563	4.036326
0.929288	130.603058	4.041331
1.032975	149.177389	4.046336
1.461908	151.009752	4.051341
0.848184	151.481076	4.056346
0.869174	141.576546	4.061350
1.082405	151.313008	4.066355
0.855225	152.899801	4.071360
1.039241	158.895863	4.076365
0.978626	159.820638	4.081370
1.066549	150.434077	4.086374
1.420117	155.084054	4.091379
1.140330	163.890422	4.096384
1.535188	154.465266	4.101389
1.388766	164.746148	4.106394
1.387871	155.675821	4.111398
0.881427	139.379099	4.116403
0.953383	162.025203	4.121408
1.196361	159.013761	4.126413
1.019707	169.657423	4.131418
1.418025	158.830406	4.136422
1.715994	160.510604	4.141427
1.353448	161.252915	4.146432
1.377501	160.627605	4.151437
1.374079	159.866933	4.156442
1.342473	162.124845	4.161446
1.274734	161.843103	4.166451
1.303036	157.021326	4.171456
1.230792	157.484287	4.176461
1.484231	160.706148	4.181466
1.386338	165.147117	4.186470
1.528852	162.337609	4.191475
1.584745	163.875554	4.196480
1.284705	150.241440	4.201485
1.399407	148.285479	4.206490
1.278270	168.742156	4.211494
1.791044	154.439252	4.216499
1.496526	160.281109	4.221504
1.321974	154.136830	4.226509
1.571435	158.106069	4.231514
1.382714	163.188818	4.236518
1.380366	164.001133	4.241523
1.179818	163.961018	4.246528
1.723807	162.047634	4.251533
1.153860	165.957003	4.256538
1.460778	167.038777	4.261542
1.535875	160.123801	4.266547
1.081300	165.248403	4.271552
1.684355	167.452330	4.276557
1.472051	168.262511	4.281562
1.468522	162.702046	4.286566
1.631375	157.880485	4.291571
1.680585	158.343265	4.296576
1.433464	159.100207	4.301581
1.753653	159.917918	4.306586
1.458630	163.003861	4.311590
1.350889	163.964660	4.316595
1.536264	176.702500	4.321600
1.748422	183.425635	4.326605
2.004808	188.105133	4.331610
2.089981	186.566689	4.336614
1.902253	162.139788	4.341619
1.681644	165.131514	4.346624
1.632838	171.526669	4.351629
2.061912	182.268950	4.356634
2.000739	173.318905	4.361638
1.983942	161.459096	4.366643
1.683196	168.415357	4.371648
1.940709	172.027272	4.376653
1.998553	169.650728	4.381658
1.618469	163.839839	4.386662
1.631380	172.737260	4.391667
1.810786	188.919224	4.396672
2.242471	192.346209	4.401677
2.192001	187.341117	4.406682
1.827052	177.161054	4.411686
1.638122	174.557785	4.416691
2.250597	193.696958	4.421696
2.225260	185.335350	4.426701
2.117673	175.980162	4.431706
1.667621	165.767232	4.436710
1.964131	173.820848	4.441715
2.246560	180.165892	4.446720
2.026266	165.878201	4.451725
1.917437	172.485565	4.456730
1.684312	190.759923	4.461734
2.430352	178.748915	4.466739
2.163769	186.748964	4.471744
1.949936	184.112718	4.476749
2.104926	188.963521	4.481754
1.808152	186.061384	4.486758
2.419940	186.398643	4.491763
2.220388	193.808609	4.496768
2.184965	183.927601	4.501773
2.079865	190.965733	4.506778
1.781014	189.930546	4.511782
2.143855	194.293651	4.516787
2.159322	195.957485	4.521792
2.130010	192.498968	4.526797
2.332728	190.323789	4.531802
1.880963	196.947103	4.536806
2.596924	198.987098	4.541811
2.259636	194.101725	4.546816
2.319253	194.958443	4.551821
2.140819	193.574552	4.556826
2.243217	198.741716	4.561830
2.278514	195.961993	4.566835
2.089105	201.126763	4.571840
2.443850	198.234744	4.576845
2.389295	195.738870	4.581850
1.949066	198.965689	4.586854
2.423126	192.595784	4.591859
2.274817	194.373962	4.596864
2.315788	192.438888	4.601869
2.374959	191.252456	4.606874
2.366092	199.860848	4.611878
2.835098	208.991399	4.616883
2.535030	211.237927	4.621888
2.732354	191.313396	4.626893
2.415026	190.587733	4.631898
2.639942	202.785448	4.636902
2.671371	188.904796	4.641907
2.152039	192.289558	4.646912
2.447563	187.914693	4.651917
2.440411	199.367013	4.656922
2.353365	202.574026	4.661926
3.015380	215.463459	4.666931
2.643348	203.050500	4.671936
2.778657	194.196374	4.676941
2.301025	196.166628	4.681946
2.371259	200.940301	4.686950
2.840824	206.183224	4.691955
2.580693	227.609817	4.696960
2.918246	218.284098	4.701965
2.654290	210.780346	4.706970
2.599029	211.435268	4.711974
2.845818	210.653684	4.716979
2.714590	205.593681	4.721984
2.554471	203.341829	4.726989
2.767122	218.761336	4.731994
3.041191	217.132605	4.736998
3.009867	206.481684	4.742003
2.445952	199.005311	4.747008
2.857303	199.478770	4.752013
2.945726	207.897993	4.757018
2.757971	201.913356	4.762022
2.796640	199.787049	4.767027
2.704849	209.222008	4.772032
2.999882	211.674285	4.777037
2.919970	212.714346	4.782042
2.690612	219.997637	4.787046
3.010285	213.920089	4.792051
2.949745	226.732634	4.797056
3.078286	219.812728	4.802061
2.905376	214.378171	4.807066
2.959425	225.113911	4.812070
3.066515	226.691535	4.817075
2.830339	226.383415	4.822080
2.885069	219.284315	4.827085
2.870045	226.341292	4.832090
2.579497	219.444410	4.837094
3.327176	212.474868	4.842099
2.785692	218.217138	4.847104
3.161389	220.386497	4.852109
3.001513	221.767774	4.857114
2.676050	224.085801	4.862118
2.763834	217.311373	4.867123
2.641045	229.707981	4.872128
2.434283	218.598286	4.877133
2.474477	229.361976	4.882138
2.942671	246.285133	4.887142
3.192853	239.722976	4.892147
3.145961	252.019021	4.897152
3.162011	252.319361	4.902157
3.160280	251.556628	4.907162
3.481298	249.203785	4.912166
3.666924	250.524498	4.917171
3.432204	250.249092	4.922176
3.425335	252.311108	4.927181
3.558327	236.727150	4.932186
3.073909	229.933803	4.937190
3.348088	228.138698	4.942195
3.388438	224.105438	4.947200
3.346411	230.630131	4.952205
2.938492	229.225235	4.957210
2.861413	236.693284	4.962214
3.498633	245.228854	4.967219
3.447082	240.900988	4.972224
3.390257	245.842731	4.977229
3.346906	245.573722	4.982234
3.438120	245.122587	4.987238
3.672713	246.020387	4.992243
3.555629	250.573686	4.997248
3.570079	244.176267	5.002253
3.297350	234.923377	5.007258
3.280442	236.192377	5.012262
3.642921	245.910105	5.017267
3.384718	249.531462	5.022272
3.594678	247.107023	5.027277
3.503692	240.279898	5.032282
3.287906	253.882658	5.037286
3.803776	245.618671	5.042291
3.372952	255.391992	5.047296
3.471786	247.078068	5.052301
3.384555	254.884267	5.057306
3.183190	248.398063	5.062310
3.402999	243.851210	5.067315
3.253762	250.075359	5.072320
3.316776	254.906880	5.077325
3.511448	247.962394	5.082330
3.162691	245.568512	5.087334
3.596585	237.013218	5.092339
3.576551	254.700017	5.097344
3.788748	250.967453	5.102349
3.925961	257.311514	5.107354
3.658816	253.997941	5.112358
4.020439	246.932272	5.117363
3.660659	254.356960	5.122368
3.924032	242.853657	5.127373
3.976285	240.787058	5.132378
3.486453	248.754644	5.137382
3.628293	244.409356	5.142387
3.542396	245.874094	5.147392
3.409430	241.366122	5.152397
3.682326	257.837760	5.157402
3.834128	264.481927	5.162406
4.489887	262.695659	5.167411
4.034077	267.760311	5.172416
3.806688	248.214673	5.177421
3.768681	249.769360	5.182426
3.547160	242.296652	5.187430
4.058302	258.318773	5.192435
4.079095	269.835784	5.197440
3.926545	258.834499	5.202445
3.851744	261.410582	5.207450
4.153412	261.334072	5.212454
4.000372	251.234508	5.217459
3.644064	256.600591	5.222464
4.179135	256.849518	5.227469
4.297540	259.527797	5.232474
4.214201	257.116404	5.237478
4.025449	251.680314	5.242483
3.569895	253.797685	5.247488
3.899742	257.751665	5.252493
4.129307	268.348651	5.257498
4.046742	267.324807	5.262502
4.497592	263.966142	5.267507
3.815994	267.886526	5.272512
4.341917	268.395678	5.277517
4.137273	270.236079	5.282522
3.960244	264.321078	5.287526
4.328742	262.200136	5.292531
3.981926	271.744261	5.297536
4.176656	277.034692	5.302541
3.944393	270.154578	5.307546
4.184694	283.528705	5.312550
4.234788	269.371381	5.317555
3.953133	281.001434	5.322560
4.321039	272.257342	5.327565
4.266808	275.189767	5.332570
4.098879	270.687576	5.337574
4.155740	270.921760	5.342579
3.652596	278.094715	5.347584
3.866665	275.365692	5.352589
4.053793	276.971903	5.357594
4.139670	278.688024	5.362598
4.259120	281.063023	5.367603
4.136795	297.875633	5.372608
4.618948	300.696746	5.377613
4.609546	305.475547	5.382618
4.313763	302.664591	5.387622
4.388681	291.861829	5.392627
4.206137	293.502024	5.397632
4.732590	297.210531	5.402637
4.654575	298.894197	5.407642
4.419046	281.919600	5.412646
4.301859	274.626543	5.417651
4.494680	293.369812	5.422656
4.445207	285.893063	5.427661
4.597017	295.886460	5.432666
4.400388	287.022323	5.437670
4.450863	291.010141	5.442675
4.506074	299.505560	5.447680
4.718535	297.933199	5.452685
4.556388	307.393485	5.457690
4.687367	311.184256	5.462694
4.750297	299.821060	5.467699
4.542601	297.004004	5.472704
5.026098	290.428252	5.477709
4.735222	284.183400	5.482714
4.243090	283.630734	5.487718
4.637291	280.172319	5.492723
4.657512	289.195287	5.497728
4.734641	293.604153	5.502733
4.632476	291.233761	5.507738
4.745959	292.569187	5.512742
4.851449	289.212649	5.517747
4.278920	291.097197	5.522752
4.480093	291.265254	5.527757
4.788637	301.094958	5.532762
4.569621	301.347987	5.537766
4.955487	292.917440	5.542771
4.785007	306.200949	5.547776
4.293691	309.372509	5.552781
4.522602	298.558254	5.557786
4.534787	307.275505	5.562790
5.122079	297.056476	5.567795
4.853311	313.800605	5.572800
4.921107	300.666873	5.577805
4.781695	306.083687	5.582810
4.964354	298.619801	5.587814
5.222236	307.921140	5.592819
4.825338	315.574205	5.597824
4.872904	307.648220	5.602829
4.918977	302.784777	5.607834
5.061598	314.539371	5.612838
5.299223	298.844683	5.617843
4.714592	301.942497	5.622848
4.773924	299.391635	5.627853
4.728067	299.397932	5.632858
4.586989	306.219082	5.637862
4.798825	298.873503	5.642867
4.646705	314.263522	5.647872
5.341671	323.647995	5.652877
5.300643	323.057728	5.657882
5.010018	321.392252	5.662886
5.174967	316.439065	5.667891
4.823399	315.577771	5.672896
5.259125	320.735561	5.677901
5.527043	323.472369	5.682906
5.024259	318.412483	5.687910
5.274929	307.436156	5.692915
5.040036	310.941579	5.697920
5.119719	307.801054	5.702925
5.068659	312.329821	5.707930
5.372267	327.079409	5.712934
5.395930	307.203023	5.717939
5.288167	315.073432	5.722944
4.967518	301.930811	5.727949
4.892071	314.445351	5.732954
5.301799	336.430739	5.737958
5.294406	332.084485	5.742963
5.507124	324.845113	5.747968
5.024971	326.132552	5.752973
5.450493	324.826835	5.757978
5.410213	331.584536	5.762982
5.519116	324.817615	5.767987
5.356566	337.448621	5.772992
5.387362	336.529534	5.777997
5.234817	333.840094	5.783002
5.196026	331.940707	5.788006
5.631407	324.980600	5.793011
5.233797	342.831259	5.798016
5.301404	329.344101	5.803021
5.511508	337.586361	5.808026
5.233132	336.402926	5.813030
5.373433	336.790834	5.818035
5.570063	340.805574	5.823040
5.402838	332.515139	5.828045
5.519772	334.862342	5.833050
5.395723	341.964264	5.838054
5.618506	330.675809	5.843059
5.499432	340.642457	5.848064
5.740598	330.785018	5.853069
5.543994	332.282699	5.858074
5.170640	345.387303	5.863078
5.803087	334.764713	5.868083
5.624014	336.103989	5.873088
5.770285	336.247195	5.878093
5.820868	334.632569	5.883098
5.184674	337.281103	5.888102
5.700932	333.717214	5.893107
5.524380	339.878433	5.898112
5.564631	335.515408	5.903117
5.704786	333.564090	5.908122
5.418326	336.307846	5.913126
5.571713	328.711642	5.918131
5.440921	337.229594	5.923136
5.489701	343.466379	5.928141
5.834258	353.142149	5.933146
6.013646	364.077657	5.938150
5.915799	349.721369	5.943155
5.417868	348.989885	5.948160
6.175482	350.510517	5.953165
6.180519	346.214495	5.958170
5.724860	344.481425	5.963174
5.735503	330.730977	5.968179
5.713753	347.337936	5.973184
5.594741	342.328949	5.978189
5.956519	351.355188	5.983194
5.957348	355.354402	5.988198
5.870923	359.859044	5.993203
5.831576	359.442155	5.998208
6.160308	351.809208	6.003213
6.256566	355.081410	6.008218
5.928405	346.595413	6.013222
5.828177	337.288243	6.018227
5.629310	345.094818	6.023232
6.053375	334.958838	6.028237
6.049614	335.031771	6.033242
5.467392	339.595024	6.038246
5.895640	346.803422	6.043251
5.959520	353.686165	6.048256
6.125019	352.381471	6.053261
5.741236	348.800854	6.058266
5.706749	347.740824	6.063270
5.930594	354.047096	6.068275
6.161896	364.256681	6.073280
5.528064	353.883429	6.078285
5.804079	350.753010	6.083290
5.681305	363.924868	6.088294
5.905519	355.430477	6.093299
5.933754	364.631938	6.098304
6.158209	367.933828	6.103309
6.157251	363.278848	6.108314
5.790070	365.909876	6.113318
6.054958	360.756206	6.118323
5.792145	373.757081	6.123328
5.799845	357.584761	6.128333
6.246580	365.588342	6.133338
5.669924	349.235731	6.138342
6.085251	350.258324	6.143347
5.797587	350.505158	6.148352
5.751264	354.256626	6.153357
6.051929	361.465437	6.158362
5.876878	365.192638	6.163366
5.950468	360.242528	6.168371
5.740387	356.715238	6.173376
5.855054	358.018899	6.178381
5.981232	362.202393	6.183386
6.034601	364.368117	6.188390
6.075095	354.676306	6.193395
5.900279	350.364085	6.198400
6.044247	344.076802	6.203405
5.725909	338.632341	6.208410
5.613088	340.724347	6.213414
6.185173	350.670484	6.218419
5.958728	346.653941	6.223424
5.951675	343.073499	6.228429
5.952589	332.060957	6.233434
5.780047	338.387079	6.238438
5.820529	328.234107	6.243443
5.892460	340.040288	6.248448
6.029845	341.966538	6.253453
5.766579	329.889294	6.258458
5.845342	353.428100	6.263462
6.084692	349.682924	6.268467
5.718907	343.797176	6.273472
5.989349	344.951309	6.278477
6.092279	347.713864	6.283482
5.846393	338.748725	6.288486
5.741985	333.054532	6.293491
5.982717	342.578171	6.298496
6.083264	344.151366	6.303501
5.893163	330.035141	6.308506
5.796810	327.976958	6.313510
5.804579	327.542795	6.318515
5.827240	335.270255	6.323520
5.639658	345.500844	6.328525
6.066489	352.775588	6.333530
5.869009	364.082140	6.338534
6.248376	355.580211	6.343539
5.830844	349.207512	6.348544
5.759501	338.540236	6.353549
5.913189	345.050329	6.358554
5.964048	358.539168	6.363558
6.029225	351.294812	6.368563
5.743957	341.510134	6.373568
6.048635	357.040639	6.378573
5.964398	341.426636	6.383578
5.854092	337.787909	6.388582
5.884815	324.817180	6.393587
5.687099	339.681962	6.398592
5.804631	351.205313	6.403597
6.125886	363.381480	6.408602
6.031593	355.323655	6.413606
5.899042	339.142412	6.418611
5.822707	341.319349	6.423616
5.855349	339.524168	6.428621
5.836592	355.756685	6.433626
6.041641	363.818244	6.438630
6.119898	346.516130	6.443635
5.921238	340.566989	6.448640
5.591531	332.985264	6.453645
6.149127	341.040924	6.458650
5.672623	345.609366	6.463654
5.797618	347.905311	6.468659
5.845478	360.976883	6.473664
6.082626	362.009445	6.478669
6.020611	354.491325	6.483674
6.184271	343.971221	6.488678
6.264626	336.452820	6.493683
5.947773	342.840730	6.498688
5.891389	336.232206	6.503693
6.033817	339.158522	6.508698
5.850932	335.552337	6.513702
5.669766	338.142297	6.518707
5.717481	336.072293	6.523712
5.978929	331.329666	6.528717
5.723699	331.882332	6.533722
5.762841	335.919795	6.538726
5.652865	330.821105	6.543731
5.668715	349.986056	6.548736
5.527076	362.457328	6.553741
5.973843	351.528419	6.558746
6.244433	364.620143	6.563750
6.496565	356.872199	6.568755
5.718759	356.770196	6.573760
5.771298	338.909934	6.578765
6.066884	351.252949	6.583770
6.172168	351.890961	6.588774
6.268804	336.345682	6.593779
5.958798	336.998786	6.598784
5.961325	339.067152	6.603789
5.898219	334.963179	6.608794
5.758381	335.103244	6.613798
6.131836	335.398473	6.618803
5.933528	339.797905	6.623808
5.843279	332.172778	6.628813
6.073389	331.386845	6.633818
5.748442	343.955946	6.638822
6.097100	334.936956	6.643827
5.980483	338.299068	6.648832
5.968026	331.064815	6.653837
6.102279	333.096567	6.658842
5.995061	341.741255	6.663846
6.061388	330.192765	6.668851
6.095956	331.559615	6.673856
5.875734	332.517145	6.678861
6.126787	332.003032	6.683866
6.018894	334.309122	6.688870
6.127843	334.674791	6.693875
5.831689	331.142619	6.698880
5.719975	334.277571	6.703885
6.251629	332.992168	6.708890
6.186452	334.106563	6.713894
5.799063	318.387675	6.718899
5.757694	318.314490	6.723904
5.843457	329.165821	6.728909
5.989661	327.490368	6.733914
5.802202	336.414748	6.738918
5.865740	328.452954	6.743923
6.118539	330.575387	6.748928
5.984803	325.469977	6.753933
6.032425	320.500302	6.758938
5.401853	324.391332	6.763942
6.005416	327.128407	6.768947
5.655910	332.743614	6.773952
5.720140	333.333958	6.778957
6.084749	328.949785	6.783962
5.661431	336.144279	6.788966
5.706222	327.622978	6.793971
5.886258	334.216322	6.798976
5.810839	333.406192	6.803981
5.851791	335.662573	6.808986
5.993013	341.056214	6.813990
6.322000	334.318361	6.818995
6.089192	339.622382	6.824000
5.926554	340.702002	6.829005
5.922817	345.059941	6.834010
5.980977	340.125219	6.839014
5.845868	341.581539	6.844019
6.063463	331.753459	6.849024
5.986651	330.013700	6.854029
6.082873	326.457996	6.859034
5.767867	329.727253	6.864038
5.924046	324.780646	6.869043
6.103924	332.093314	6.874048
5.890223	315.808906	6.879053
5.865229	305.006696	6.884058
5.500164	313.393323	6.889062
6.067782	325.306066	6.894067
5.629823	330.200637	6.899072
6.050393	328.079549	6.904077
6.036103	335.623682	6.909082
5.578612	340.829536	6.914086
6.246957	336.146022	6.919091
5.950053	330.388983	6.924096
5.786735	334.740192	6.929101
6.286339	334.968946	6.934106
5.591479	333.050324	6.939110
6.176639	324.786267	6.944115
5.949683	328.584019	6.949120
5.909619	312.132331	6.954125
5.734630	304.402452	6.959130
5.770809	324.932152	6.964134
5.903293	320.202398	6.969139
5.872458	336.971879	6.974144
6.169821	340.223604	6.979149
5.696520	316.573505	6.984154
5.330818	329.285901	6.989158
5.949373	335.552063	6.994163
6.304957	335.560559	6.999168
6.052887	335.804261	7.004173
6.160845	329.030391	7.009178
5.758829	323.471127	7.014182
6.141750	318.226686	7.019187
5.600974	323.042769	7.024192
5.864273	319.335273	7.029197
6.024459	324.320041	7.034202
5.623571	342.497048	7.039206
6.016560	325.197701	7.044211
5.918697	335.350080	7.049216
6.078045	334.402602	7.054221
5.965709	333.680086	7.059226
5.706025	331.858916	7.064230
6.055622	328.136733	7.069235
6.134196	335.479399	7.074240
5.730480	321.294164	7.079245
5.812061	315.279683	7.084250
5.873088	338.484942	7.089254
5.769832	330.245878	7.094259
5.928431	335.235057	7.099264
5.836198	339.416427	7.104269
6.223875	336.087548	7.109274
5.584391	333.477359	7.114278
5.920782	337.442314	7.119283
5.696198	340.209175	7.124288
5.784452	339.125071	7.129293
5.837319	333.088105	7.134298
5.691406	337.952472	7.139302
6.053559	333.609356	7.144307
5.827534	339.038945	7.149312
5.684918	339.387071	7.154317
6.001370	339.638852	7.159322
5.809112	338.872539	7.164326
6.041998	337.879730	7.169331
5.888087	331.659145	7.174336
6.110756	344.066918	7.179341
6.084206	335.302464	7.184346
6.006485	347.581194	7.189350
5.950452	335.961791	7.194355
5.893941	338.827511	7.199360
6.168983	337.972173	7.204365
6.248943	339.534371	7.209370
5.749414	326.179018	7.214374
5.695298	320.936497	7.219379
5.720191	329.441689	7.224384
5.593032	339.496306	7.229389
5.948111	345.230663	7.234394
5.928109	343.986880	7.239398
6.092206	342.245512	7.244403
5.841582	339.979618	7.249408
5.707269	333.348480	7.254413
6.077685	337.608544	7.259418
5.485564	339.568371	7.264422
5.782800	335.009657	7.269427
5.954030	338.462833	7.274432
5.800785	340.514960	7.279437
5.982887	337.577305	7.284442
5.899029	340.591610	7.289446
6.090642	330.124313	7.294451
5.830422	341.437488	7.299456
5.758502	337.406016	7.304461
6.100858	336.014217	7.309466
5.917104	339.324496	7.314470
5.720724	339.522074	7.319475
5.945073	332.421870	7.324480
5.796207	333.120122	7.329485
6.197849	331.513471	7.334490
5.952434	333.516528	7.339494
5.932975	329.370598	7.344499
5.781206	335.585926	7.349504
5.903052	335.292718	7.354509
6.079514	325.858038	7.359514
5.966147	336.137901	7.364518
6.245214	332.866080	7.369523
5.754790	344.601990	7.374528
5.912630	336.018945	7.379533
6.170577	333.860847	7.384538
5.782260	345.311667	7.389542
5.965692	334.758497	7.394547
5.795139	338.391014	7.399552
6.177537	330.256634	7.404557
5.966400	334.251474	7.409562
5.895076	332.836613	7.414566
5.595345	322.723602	7.419571
5.656455	328.522221	7.424576
5.712820	339.749424	7.429581
6.090208	329.765233	7.434586
5.804996	344.218651	7.439590
5.895193	331.230372	7.444595
5.775094	332.026674	7.449600
5.684062	338.071707	7.454605
6.011690	339.951456	7.459610
5.919387	336.719028	7.464614
5.746454	333.555208	7.469619
5.943541	329.836967	7.474624
5.860732	326.460688	7.479629
6.096721	326.208175	7.484634
5.419763	337.332632	7.489638
5.847196	335.694872	7.494643
5.396353	338.507684	7.499648
5.415231	339.324387	7.504653
5.760119	335.695534	7.509658
5.504321	351.030730	7.514662
6.088939	358.468201	7.519667
6.086945	367.224934	7.524672
6.483806	357.981863	7.529677
6.038677	347.015347	7.534682
5.855286	343.374710	7.539686
5.891559	333.038315	7.544691
5.761789	342.247574	7.549696
5.909429	340.477160	7.554701
6.001758	334.978708	7.559706
5.968272	333.202569	7.564710
5.958297	329.089602	7.569715
5.786026	334.524892	7.574720
5.647788	338.161924	7.579725
5.946128	333.209929	7.584730
5.779724	335.196351	7.589734
6.011973	330.369165	7.594739
6.099468	343.397651	7.599744
5.681233	338.889725	7.604749
5.961659	333.557465	7.609754
6.002232	333.027095	7.614758
5.805184	339.517513	7.619763
5.672827	334.884300	7.624768
5.585837	341.685459	7.629773
6.058293	344.321306	7.634778
5.963134	342.535447	7.639782
5.865232	337.704517	7.644787
5.992842	335.078405	7.649792
5.900287	340.388803	7.654797
5.842023	332.148406	7.659802
5.976584	350.355751	7.664806
6.122416	328.442701	7.669811
6.082455	333.436342	7.674816
5.483493	333.919631	7.679821
6.241625	335.934902	7.684826
5.946566	338.265474	7.689830
5.859135	331.491199	7.694835
5.442075	335.285701	7.699840
5.508142	343.975106	7.704845
6.407751	350.383390	7.709850
5.902340	359.863647	7.714854
5.772651	346.066566	7.719859
5.755211	346.222279	7.724864
6.062385	359.730442	7.729869
6.168715	355.582224	7.734874
5.783463	348.307670	7.739878
5.957209	342.988534	7.744883
5.902624	342.135682	7.749888
5.579747	343.729855	7.754893
5.979478	355.739097	7.759898
5.938756	362.206401	7.764902
6.135516	362.183771	7.769907
5.952239	351.650070	7.774912
5.895309	341.868627	7.779917
6.034255	335.829247	7.784922
5.732869	335.903709	7.789926
5.682327	335.327251	7.794931
5.887381	349.141022	7.799936
6.186091	355.310574	7.804941
6.164469	347.080086	7.809946
5.979411	345.645378	7.814950
6.090159	335.123780	7.819955
5.843868	346.135093	7.824960
5.945906	342.248866	7.829965
6.093661	338.864006	7.834970
5.876605	335.823723	7.839974
6.043290	339.282980	7.844979
5.757436	343.188763	7.849984
6.023862	351.227325	7.854989
6.066009	343.511200	7.859994
5.883413	345.388216	7.864998
6.078049	333.060697	7.870003
5.824901	337.978145	7.875008
5.876858	338.603083	7.880013
5.943911	338.917278	7.885018
5.834785	339.251175	7.890022
5.739922	337.656094	7.895027
5.614419	332.720016	7.900032
5.770290	334.961708	7.905037
6.116188	341.163697	7.910042
5.752775	339.685509	7.915046
5.909641	336.579164	7.920051
6.058973	334.644876	7.925056
5.747506	342.473254	7.930061
6.147431	329.386919	7.935066
6.073682	346.049849	7.940070
6.069494	343.889375	7.945075
5.892058	342.586806	7.950080
5.937653	337.327768	7.955085
6.155689	334.033492	7.960090
6.044078	343.412811	7.965094
6.355113	340.511230	7.970099
6.088184	344.386055	7.975104
5.533434	337.409335	7.980109
6.104859	344.833592	7.985114
5.883631	344.755460	7.990118
6.105149	338.330849	7.995136
6.069354	332.371185	8.000154
5.775128	340.164073	8.005171
6.173945	335.388248	8.010189
6.098910	342.274436	8.015206
5.915029	325.414556	8.020224
5.790920	330.358822	8.025242
5.555787	336.885329	8.030259
6.081976	330.658012	8.035277
5.968749	332.362935	8.040294
6.083321	338.953573	8.045312
5.724649	342.078758	8.050330
5.618793	347.619763	8.055347
5.966699	336.184183	8.060365
5.804581	343.013341	8.065382
5.831508	336.670483	8.070400
5.801715	334.543384	8.075418
6.166171	343.363530	8.080435
6.332139	328.904579	8.085453
5.955671	341.753802	8.090470
6.232629	339.492646	8.095488
6.105382	339.137060	8.100506
5.605055	345.402390	8.105523
6.233041	344.232820	8.110541
5.804855	339.515204	8.115558
5.962084	344.680976	8.120576
5.720314	332.533067	8.125594
5.590202	336.837238	8.130611
5.961258	332.941532	8.135629
5.569422	342.900811	8.140646
5.813509	331.545019	8.145664
6.265638	343.678538	8.150682
6.145732	359.812987	8.155699
5.860647	347.052208	8.160717
6.176869	360.159155	8.165734
6.306658	352.472194	8.170752
6.209808	341.335043	8.175770
6.206692	344.918044	8.180787
6.488798	333.899629	8.185805
6.011318	346.247907	8.190822
6.111710	337.133254	8.195840
6.099844	333.862331	8.200858
5.778944	338.177033	8.205875
5.759922	333.617041	8.210893
6.113077	347.747506	8.215910
6.341651	360.217245	8.220928
6.502778	351.975530	8.225946
5.684387	342.954951	8.230963
6.002796	334.232118	8.235981
6.209263	355.775873	8.240998
6.352725	353.070714	8.246016
6.303345	349.655420	8.251034
6.086670	346.888451	8.256051
6.099588	331.605104	8.261069
5.829546	347.607131	8.266086
6.187134	352.148042	8.271104
6.258622	362.246539	8.276122
6.318871	367.347085	8.281139
6.483676	358.800647	8.286157
6.028792	361.813037	8.291174
6.426221	358.661917	8.296192
6.079189	343.671609	8.301210
5.990540	355.382126	8.306227
6.464039	353.173258	8.311245
6.441581	365.153313	8.316262
5.995420	356.065969	8.321280
6.330341	352.972441	8.326298
6.176914	361.317768	8.331315
6.429774	361.570447	8.336333
6.340269	358.298990	8.341350
5.977335	349.844473	8.346368
6.221775	355.352277	8.351386
6.372106	363.947479	8.356403
6.405147	358.717294	8.361421
6.240996	368.306432	8.366438
6.294769	357.200426	8.371456
6.416537	364.380585	8.376474
6.372328	367.336979	8.381491
6.001673	355.419041	8.386509
6.250621	364.631132	8.391526
6.270875	358.822400	8.396544
6.608288	353.550083	8.401562
6.257815	358.138959	8.406579
6.489776	358.931671	8.411597
6.579636	359.070408	8.416614
6.096172	345.530337	8.421632
6.280287	348.905971	8.426650
6.557847	358.981167	8.431667
6.427682	348.201864	8.436685
6.192322	349.005037	8.441702
6.207761	355.598909	8.446720
6.454889	362.142805	8.451738
6.327233	363.683401	8.456755
6.667236	361.669065	8.461773
6.546435	363.197897	8.466790
5.974972	344.443468	8.471808
6.512698	352.181859	8.476826
6.195079	358.546851	8.481843
6.800547	353.191369	8.486861
6.489172	361.109736	8.491878
6.618256	356.565956	8.496896
6.365973	340.232899	8.501914
5.945762	344.980945	8.506931
6.665199	358.321886	8.511949
6.747519	359.830270	8.516966
6.408678	359.561686	8.521984
6.080214	365.439931	8.527002
6.331966	370.563684	8.532019
6.602100	369.864362	8.537037
6.484919	361.279781	8.542054
6.341372	362.155933	8.547072
6.595701	360.183735	8.552090
6.232533	370.599077	8.557107
6.615731	359.800696	8.562125
6.771983	363.894672	8.567143
6.607142	363.355954	8.572160
6.753069	354.362679	8.577178
6.493891	362.043680	8.582195
6.453679	363.093848	8.587213
6.564324	366.376738	8.592231
6.568160	368.843520	8.597248
6.934752	361.021680	8.602266
6.506865	357.764133	8.607283
6.305881	348.461602	8.612301
6.498749	356.132111	8.617319
5.992111	354.081412	8.622336
6.253148	354.715188	8.627354
6.206843	367.071408	8.632371
6.380079	350.858807	8.637389
6.409322	361.596534	8.642407
6.593044	372.431710	8.647424
6.830733	356.567655	8.652442
6.363679	364.450390	8.657459
6.470405	359.305830	8.662477
6.473420	366.048800	8.667495
6.548618	368.452391	8.672512
6.607835	364.581546	8.677530
6.443246	367.331513	8.682547
6.791455	379.221855	8.687565
6.710679	372.299814	8.692583
6.398434	377.067194	8.697600
6.870282	380.393220	8.702618
6.655328	385.552531	8.707635
6.352123	380.453210	8.712653
6.905301	379.146036	8.717671
6.791323	391.885699	8.722688
7.158378	379.850306	8.727706
6.744261	372.966733	8.732723
6.481718	365.475037	8.737741
6.523104	368.668419	8.742759
6.459295	366.846139	8.747776
6.884468	371.141432	8.752794
6.816914	380.896852	8.757811
6.350905	380.973120	8.762829
6.761858	385.104053	8.767847
6.831330	392.990077	8.772864
6.960546	380.107520	8.777882
6.879408	390.175014	8.782899
6.917350	389.169284	8.787917
7.053306	368.946798	8.792935
6.489867	363.252435	8.797952
6.654022	371.652257	8.802970
6.604468	372.012883	8.807987
6.698513	376.984617	8.813005
6.747578	390.091934	8.818023
6.817760	385.409486	8.823040
6.757529	386.465333	8.828058
6.771792	391.169595	8.833075
7.013031	390.037688	8.838093
6.899965	389.582515	8.843111
6.977936	400.552734	8.848128
7.034523	387.419618	8.853146
6.712159	373.997717	8.858163
6.676897	376.008214	8.863181
7.053277	385.438569	8.868199
6.903103	387.894836	8.873216
7.143064	369.067621	8.878234
6.453892	373.511224	8.883251
6.164515	386.407082	8.888269
6.566181	388.329089	8.893287
6.722726	392.615725	8.898304
6.711214	394.875030	8.903322
6.859360	387.147809	8.908339
6.821931	389.249408	8.913357
7.346801	394.443092	8.918375
7.138554	395.504947	8.923392
7.231290	384.902274	8.928410
7.242451	393.828193	8.933427
6.895372	398.060639	8.938445
7.440182	393.953483	8.943463
7.194193	394.578904	8.948480
7.198900	386.149309	8.953498
6.567635	376.916437	8.958515
6.646672	379.246958	8.963533
6.985148	387.369123	8.968551
6.877873	397.453153	8.973568
7.053574	394.584590	8.978586
6.962793	397.395563	8.983603
7.074590	398.773489	8.988621
7.146471	386.569663	8.993639
7.030599	396.749598	8.998656
7.055782	386.345891	9.003674
6.754134	388.144025	9.008691
7.083069	394.440940	9.013709
7.413336	387.549049	9.018727
6.898418	399.315817	9.023744
7.262636	391.739218	9.028762
7.029494	399.555286	9.033779
6.768046	390.244240	9.038797
7.011514	387.171754	9.043815
7.049333	389.386080	9.048832
7.315806	398.065605	9.053850
7.346555	389.602367	9.058867
7.112480	392.129217	9.063885
7.253377	388.521985	9.068903
6.837227	390.305420	9.073920
6.980726	380.840716	9.078938
6.797688	384.728302	9.083955
6.768792	387.948286	9.088973
6.937184	377.796442	9.093991
6.734022	389.989101	9.099008
6.973237	383.942739	9.104026
7.181561	380.648138	9.109043
7.131924	391.669006	9.114061
7.207574	388.757961	9.119079
6.922697	400.739374	9.124096
7.147264	386.400184	9.129114
7.047232	398.598803	9.134131
6.954530	399.371073	9.139149
7.208610	389.796720	9.144167
7.132088	398.776134	9.149184
6.976415	402.541879	9.154202
7.261385	405.542189	9.159219
7.492008	423.368925	9.164237
7.769065	411.065558	9.169255
7.301594	404.892132	9.174272
6.910737	396.284744	9.179290
7.191062	388.444500	9.184307
7.003532	398.181415	9.189325
7.816453	391.035201	9.194343
7.158802	394.963787	9.199360
7.123925	396.550042	9.204378
7.057901	394.889923	9.209395
7.131078	406.898462	9.214413
7.596872	411.261051	9.219431
7.180101	403.449625	9.224448
7.127402	405.222676	9.229466
7.475232	408.590306	9.234483
7.182249	415.773622	9.239501
7.504060	410.360966	9.244519
7.358339	415.488156	9.249536
7.381184	402.241923	9.254554
7.230955	395.204808	9.259571
7.425630	412.112355	9.264589
7.404802	408.533080	9.269607
7.296942	407.851865	9.274624
7.118565	404.676604	9.279642
7.509776	410.791376	9.284659
7.473103	414.939161	9.289677
7.731883	411.652733	9.294695
7.662324	407.526844	9.299712
6.930299	391.661924	9.304730
7.089559	403.328670	9.309747
7.195519	413.392164	9.314765
7.575724	420.539396	9.319783
7.446129	416.876169	9.324800
7.856582	426.718199	9.329818
7.639668	417.126947	9.334835
7.332170	394.906356	9.339853
7.487140	384.502418	9.344871
7.255508	395.456976	9.349888
7.635692	406.627333	9.354906
7.646477	401.279962	9.359923
7.438048	410.436530	9.364941
7.629692	392.831174	9.369959
7.189859	390.592453	9.374976
7.665023	399.592119	9.379994
7.463011	388.811890	9.385011
7.512471	403.396406	9.390029
7.504125	386.491251	9.395047
7.472236	399.192525	9.400064
7.417480	410.787834	9.405082
7.849503	412.846932	9.410099
7.720703	402.073664	9.415117
7.459479	395.134647	9.420135
7.309107	395.017911	9.425152
7.343847	398.226966	9.430170
7.930863	415.726587	9.435187
7.267048	413.830245	9.440205
7.716213	416.093577	9.445223
7.572441	421.300164	9.450240
7.717546	423.609517	9.455258
7.624431	410.481487	9.460275
7.200014	420.000574	9.465293
7.868030	415.012049	9.470311
7.694434	430.929495	9.475328
7.685475	424.531524	9.480346
7.805140	419.097028	9.485363
7.612316	416.901449	9.490381
7.654813	410.751047	9.495399
7.686237	423.293835	9.500416
7.690869	423.436253	9.505434
7.703020	407.877977	9.510451
7.594148	410.165806	9.515469
7.530037	410.077499	9.520487
7.558838	419.251674	9.525504
7.399663	421.140384	9.530522
7.666316	418.374266	9.535539
7.590488	423.109006	9.540557
7.757123	420.729306	9.545575
7.796130	415.717783	9.550592
7.586237	428.051735	9.555610
7.847121	416.469100	9.560627
7.785438	424.352254	9.565645
7.995057	417.500405	9.570663
7.655621	422.600230	9.575680
7.670036	424.841269	9.580698
7.867459	416.355732	9.585715
7.710207	420.118199	9.590733
7.858290	416.479065	9.595751
7.935080	415.193692	9.600768
7.575444	431.904882	9.605786
7.874441	422.751387	9.610803
7.741543	424.092281	9.615821
7.986523	414.100946	9.620839
7.739630	423.276685	9.625856
7.765505	420.763612	9.630874
7.886665	418.810309	9.635891
7.768509	419.362007	9.640909
7.842820	415.927398	9.645927
8.153520	417.773533	9.650944
7.945426	420.198061	9.655962
7.773174	428.332777	9.660979
7.936720	422.333770	9.665997
7.671983	423.110711	9.671015
7.649963	421.498615	9.676032
7.811432	423.913714	9.681050
7.805931	414.191006	9.686067
7.750027	424.013219	9.691085
7.843455	423.535071	9.696103
8.002446	422.203608	9.701120
7.829251	428.094351	9.706138
7.810411	414.001923	9.711155
7.895526	427.556616	9.716173
7.816886	407.980397	9.721191
7.746690	420.781332	9.726208
7.652240	419.094818	9.731226
8.095761	433.583796	9.736243
8.170255	445.991921	9.741261
8.221195	431.358629	9.746279
8.077809	424.646722	9.751296
7.906322	432.579359	9.756314
8.075871	418.284287	9.761331
7.842153	419.787731	9.766349
7.921842	429.752444	9.771367
8.244789	436.985538	9.776384
7.991062	437.840375	9.781402
8.022007	422.378375	9.786419
7.889761	430.072837	9.791437
8.311219	444.789282	9.796455
8.366782	439.593133	9.801472
8.108844	435.495281	9.806490
8.170992	423.193832	9.811507
7.976237	425.359871	9.816525
7.964926	419.971274	9.821543
7.971707	425.956614	9.826560
7.752425	440.225259	9.831578
8.387076	451.634593	9.836595
8.381690	453.869468	9.841613
8.243757	445.598687	9.846631
8.219241	429.252030	9.851648
7.875633	433.809281	9.856666
8.442558	432.750596	9.861683
7.805717	438.025059	9.866701
8.329612	441.509200	9.871719
8.328158	445.606282	9.876736
8.012771	445.072413	9.881754
8.282165	441.028173	9.886771
8.539364	448.598711	9.891789
8.112972	432.376664	9.896807
8.079214	432.107950	9.901824
8.075476	441.261740	9.906842
8.577406	443.868479	9.911859
8.485345	444.786894	9.916877
8.101212	430.298477	9.921895
8.093686	438.647243	9.926912
8.292188	444.489040	9.931930
8.612951	443.379588	9.936947
8.150099	431.961271	9.941965
7.853821	431.526003	9.946983
8.344271	436.999988	9.952000
8.257718	448.089209	9.957018
8.665210	439.275981	9.962035
8.511501	440.861644	9.967053
8.280020	439.773368	9.972071
8.238154	430.082654	9.977088
8.301439	438.883047	9.982106
8.637382	435.045883	9.987123
8.388502	430.630413	9.992141
7.943817	434.623538	9.997159
8.260891	431.920324	10.002176
8.452275	457.326284	10.007194
8.760045	450.684726	10.012211
8.394657	443.547203	10.017229
8.099362	432.203889	10.022247
8.668029	437.287193	10.027264
8.582822	440.589145	10.032282
8.305856	424.937793	10.037299
8.327105	432.146833	10.042317
8.561006	447.403947	10.047335
8.532950	433.546672	10.052352
8.072688	433.527507	10.057370
8.138952	436.377635	10.062387
8.484676	445.173581	10.067405
8.294532	446.738705	10.072423
8.415122	441.338691	10.077440
8.429036	453.437388	10.082458
8.550332	446.968630	10.087475
8.517830	439.848618	10.092493
8.555357	447.772832	10.097511
8.779496	443.982327	10.102528
8.377553	448.496490	10.107546
8.660390	447.069129	10.112563
8.697386	444.784705	10.117581
8.209592	457.109781	10.122599
8.590350	443.631029	10.127616
8.267863	450.023437	10.132634
8.406508	442.010184	10.137651
8.435440	457.849636	10.142669
8.366516	452.601858	10.147687
8.569857	449.515927	10.152704
8.562605	449.469578	10.157722
8.932901	448.970581	10.162739
8.839990	451.493945	10.167757
8.191884	453.883277	10.172775
8.744228	451.135983	10.177792
8.709326	451.641616	10.182810
8.862921	443.962083	10.187827
8.736821	448.408720	10.192845
8.706890	445.214972	10.197863
8.568394	443.862891	10.202880
8.593930	449.683729	10.207898
8.837026	440.314693	10.212915
8.822605	443.308489	10.217933
8.587823	447.701671	10.222951
8.763082	443.429925	10.227968
8.468625	446.618507	10.232986
8.602815	445.993265	10.238003
8.612819	441.190065	10.243021
8.284865	445.170949	10.248039
8.732792	451.070455	10.253056
8.661359	466.064982	10.258074
9.094611	469.300378	10.263091
8.560658	448.449401	10.268109
8.488787	460.595968	10.273127
9.094036	467.076473	10.278144
9.072411	471.567426	10.283162
8.785745	452.736573	10.288179
8.774886	461.028032	10.293197
8.758460	448.065016	10.298215
9.179066	456.893645	10.303232
8.802982	456.544027	10.308250
8.477349	452.060164	10.313267
8.738009	462.527766	10.318285
8.562273	474.982665	10.323303
8.957433	467.456611	10.328320
8.800325	471.318863	10.333338
8.980613	474.751650	10.338355
8.755720	471.502194	10.343373
8.674015	485.140266	10.348391
9.213441	471.162808	10.353408
9.086883	482.209075	10.358426
9.216709	471.116377	10.363443
9.589032	482.232386	10.368461
9.060532	465.247935	10.373479
9.024650	447.126887	10.378496
8.654242	449.191710	10.383514
8.609206	446.536842	10.388531
8.670296	455.472637	10.393549
9.027687	467.821731	10.398567
9.105752	476.575803	10.403584
8.740619	479.425726	10.408602
8.579585	476.947531	10.413619
8.910147	472.485110	10.418637
8.874076	472.687415	10.423655
9.017243	479.211373	10.428672
9.189438	480.221258	10.433690
9.053873	476.184031	10.438707
9.275760	482.190266	10.443725
9.243305	481.542226	10.448743
9.465192	478.610886	10.453760
9.340431	472.409617	10.458778
9.169471	476.509975	10.463795
9.466311	476.533933	10.468813
8.764635	468.784414	10.473831
9.158995	468.377881	10.478848
9.238089	473.018287	10.483866
8.692322	470.865397	10.488883
9.268180	474.152372	10.493901
9.091895	478.021344	10.498919
9.389915	464.444472	10.503936
9.302274	467.923593	10.508954
9.167479	471.179042	10.513971
9.328156	469.688252	10.518989
9.000775	478.705906	10.524007
8.956841	469.273366	10.529024
8.900421	467.107354	10.534042
8.994581	469.353108	10.539059
9.349689	467.284686	10.544077
8.980813	472.454359	10.549095
9.256718	475.945323	10.554112
9.258590	481.388622	10.559130
9.379085	478.528398	10.564147
9.419995	476.061051	10.569165
9.224535	477.537104	10.574183
9.453807	471.237056	10.579200
9.518946	472.442019	10.584218
9.323940	471.155392	10.589235
9.160188	462.737313	10.594253
9.100879	468.938521	10.599271
9.381883	471.089560	10.604288
9.132009	467.859791	10.609306
9.203985	468.123332	10.614323
9.423135	460.399868	10.619341
9.158749	465.909494	10.624359
9.595502	463.204172	10.629376
9.562364	471.252296	10.634394
9.107535	472.414236	10.639411
9.473508	463.142153	10.644429
9.161108	462.709357	10.649447
9.416180	464.406059	10.654464
9.521277	467.638712	10.659482
9.450434	468.011330	10.664499
9.808545	471.451478	10.669517
9.269819	474.109098	10.674535
9.490258	470.499109	10.679552
9.237769	471.550579	10.684570
9.225635	473.314363	10.689587
9.219953	468.495053	10.694605
8.994950	478.341759	10.699623
9.521459	488.403571	10.704640
9.684663	487.075538	10.709658
9.439240	484.284960	10.714675
9.752326	479.965579	10.719693
9.493645	485.610675	10.724711
9.479560	475.805497	10.729728
9.466496	481.053251	10.734746
9.322011	488.774177	10.739763
9.602341	490.350763	10.744781
9.496495	491.563176	10.749799
9.596062	482.902677	10.754816
9.680490	496.701622	10.759834
9.428582	502.937295	10.764851
9.781808	490.315368	10.769869
9.564923	499.831434	10.774887
9.909656	491.298629	10.779904
10.040761	495.828271	10.784922
9.400978	483.204849	10.789939
9.678123	479.550233	10.794957
9.639191	474.830909	10.799975
9.574797	479.319499	10.804992
9.835140	481.489313	10.810010
9.385800	487.102403	10.815027
9.792512	481.550672	10.820045
9.623052	497.742877	10.825063
9.850995	493.616516	10.830080
9.747578	494.021889	10.835098
9.808045	497.836900	10.840115
10.111155	488.042374	10.845133
9.586340	486.701508	10.850151
9.607917	479.845536	10.855168
9.868997	489.519244	10.860186
9.684428	490.296889	10.865203
9.557780	480.248948	10.870221
9.634638	493.546422	10.875239
9.638867	487.757224	10.880256
9.667310	495.080054	10.885274
9.614276	492.412331	10.890291
10.096735	489.570507	10.895309
9.701070	495.261714	10.900327
9.854040	494.755398	10.905344
9.668549	485.755316	10.910362
9.704533	496.017840	10.915379
9.653450	490.075803	10.920397
9.610283	491.452234	10.925415
9.454341	484.449880	10.930432
9.694893	491.227581	10.935450
9.854762	508.519909	10.940467
10.076181	509.491136	10.945485
10.195567	511.024891	10.950503
10.055138	495.840589	10.955520
10.063570	489.269250	10.960538
9.736033	486.550139	10.965555
9.875277	490.878445	10.970573
9.688486	497.415320	10.975591
9.503831	508.058262	10.980608
9.959038	516.181045	10.985626
10.134476	525.047949	10.990643
10.455767	521.387785	10.995661
10.168438	515.847236	11.000679
10.105667	517.877266	11.005696
10.349450	519.601433	11.010714
10.017774	507.189553	11.015731
9.949719	497.751935	11.020749
9.968893	501.241917	11.025767
10.050963	517.975326	11.030784
9.983836	515.110930	11.035802
9.686668	522.244991	11.040819
10.304414	520.331091	11.045837
10.354596	518.499759	11.050855
10.249591	515.246188	11.055872
10.331220	517.324744	11.060890
10.345576	511.832658	11.065907
10.493277	495.846363	11.070925
10.353684	489.290088	11.075943
10.029614	490.415023	11.080960
10.066788	480.997783	11.085978
9.883090	490.191638	11.090995
9.824129	496.184546	11.096013
10.534353	503.397830	11.101031
10.067626	503.269309	11.106048
10.562591	506.541538	11.111066
10.113923	511.293166	11.116083
10.047441	499.471587	11.121101
10.143172	508.594183	11.126119
10.372125	519.699317	11.131136
10.488048	516.585922	11.136154
10.221359	511.376580	11.141171
10.579580	505.075638	11.146189
10.107347	506.265657	11.151207
10.174570	507.984613	11.156224
10.370130	497.697295	11.161242
10.550634	511.977358	11.166259
10.599560	502.312703	11.171277
10.266876	500.047561	11.176295
10.248823	495.297019	11.181312
10.310193	486.888889	11.186330
9.978759	499.650674	11.191347
10.201693	507.104875	11.196365
10.266322	510.998525	11.201383
10.257419	511.378406	11.206400
10.626947	512.366443	11.211418
10.315955	514.106102	11.216435
10.592283	511.532645	11.221453
10.697059	515.891271	11.226471
10.387620	517.512571	11.231488
10.688774	504.779380	11.236506
10.391760	519.657976	11.241523
10.632551	513.465643	11.246541
10.598492	519.398731	11.251559
10.491663	520.024340	11.256576
10.720730	503.981849	11.261594
10.154105	514.748869	11.266611
10.356108	517.364738	11.271629
10.608516	519.909076	11.276647
10.474928	517.822760	11.281664
10.859328	514.315522	11.286682
10.627844	518.494413	11.291699
10.551100	517.751744	11.296717
10.503840	512.880057	11.301735
10.532511	525.444249	11.306752
10.595643	512.610908	11.311770
10.712579	519.613605	11.316787
10.646813	521.232939	11.321805
10.490654	513.280867	11.326823
10.149708	519.384056	11.331840
10.532905	519.933245	11.336858
10.499422	517.490414	11.341875
10.468562	511.872754	11.346893
10.520870	516.236722	11.351911
10.461597	515.041977	11.356928
10.886440	513.625148	11.361946
10.391166	515.886629	11.366963
10.258880	523.319941	11.371981
10.372613	539.007057	11.376999
10.434346	546.649969	11.382016
11.110441	539.653897	11.387034
11.135459	540.514350	11.392051
11.332660	532.849205	11.397069
11.230660	524.721634	11.402087
10.808114	521.177754	11.407104
10.786127	514.405943	11.412122
10.859370	521.370604	11.417139
10.779239	516.340590	11.422157
10.721084	514.090219	11.427175
10.611615	516.800772	11.432192
10.968566	512.903421	11.437210
11.024821	514.161036	11.442227
11.187046	505.538767	11.447245
11.195164	509.658099	11.452263
10.705206	515.196434	11.457280
11.344364	513.089238	11.462298
10.806564	517.370226	11.467315
10.912234	513.670380	11.472333
10.681187	511.281720	11.477351
10.853125	518.748900	11.482368
10.942451	507.568793	11.487386
10.754348	517.529681	11.492403
11.007832	513.495143	11.497421
11.068635	515.204730	11.502439
10.923949	521.472062	11.507456
10.872319	515.718282	11.512474
10.426211	518.826093	11.517491
10.922802	529.851484	11.522509
11.060431	541.736470	11.527527
11.479416	542.174622	11.532544
11.197386	527.006847	11.537562
11.305961	527.045445	11.542579
11.215867	515.245283	11.547597
11.052923	512.304437	11.552615
10.612329	526.050987	11.557632
11.175265	517.959562	11.562650
11.060800	518.503567	11.567667
11.158266	530.426688	11.572685
11.187535	515.428032	11.577703
10.931525	531.707434	11.582720
11.158423	532.838374	11.587738
11.049818	539.348147	11.592755
11.234521	540.723462	11.597773
11.637829	532.034488	11.602791
11.245918	536.183456	11.607808
11.410223	522.015526	11.612826
11.354937	512.543700	11.617843
10.813203	517.198937	11.622861
11.246252	513.884811	11.627879
11.154667	537.702830	11.632896
11.395908	535.459961	11.637914
11.434355	541.512736	11.642931
11.209522	530.825551	11.647949
11.462887	523.780400	11.652967
11.130725	524.232705	11.657984
11.482025	523.791573	11.663002
11.403276	520.660023	11.668019
11.402058	520.090269	11.673037
10.990611	511.540553	11.678055
11.363297	534.082751	11.683072
11.469711	530.213301	11.688090
11.500518	542.734833	11.693107
11.252329	541.096990	11.698125
11.516540	535.177721	11.703143
11.148755	539.325057	11.708160
11.355976	534.514760	11.713178
11.314595	544.519082	11.718195
11.615950	545.688478	11.723213
11.928271	541.417432	11.728231
11.351132	544.644380	11.733248
11.769839	533.055011	11.738266
11.187222	521.279319	11.743283
11.137704	535.949045	11.748301
11.399976	534.083772	11.753319
11.053824	539.771519	11.758336
11.216748	529.612608	11.763354
11.452993	539.407972	11.768371
11.239284	536.607015	11.773389
11.332491	534.870124	11.778407
11.585611	542.722271	11.783424
11.526092	532.958830	11.788442
11.720509	536.696949	11.793459
11.448949	542.855779	11.798477
11.734101	540.802476	11.803495
11.334309	546.037721	11.808512
11.516100	541.290290	11.813530
11.566600	541.052894	11.818547
11.842110	545.626744	11.823565
11.877473	549.169564	11.828583
11.898637	543.260225	11.833600
12.055989	545.214441	11.838618
11.933118	532.156586	11.843635
11.856024	540.243716	11.848653
11.881520	536.229602	11.853671
11.786475	536.717442	11.858688
11.481417	541.116186	11.863706
11.644902	536.970962	11.868723
11.820854	536.921046	11.873741
11.977971	534.283866	11.878759
11.643332	546.788953	11.883776
11.531314	531.812101	11.888794
11.746551	534.172452	11.893811
11.500837	544.746007	11.898829
11.639919	532.562826	11.903847
11.469060	545.604534	11.908864
11.975036	556.302821	11.913882
12.224271	556.153768	11.918899
12.064037	548.947384	11.923917
11.945933	538.562578	11.928935
11.751958	537.145271	11.933952
11.673896	534.727338	11.938970
12.057711	533.706449	11.943987
12.160345	539.397042	11.949005
12.137240	532.882085	11.954023
11.674914	541.561318	11.959040
11.962058	533.137626	11.964058
11.987221	534.258275	11.969075
11.733985	533.403895	11.974093
12.217847	522.858991	11.979111
12.060947	539.491256	11.984128
12.024409	524.279093	11.989146
11.945110	532.674044	11.994163
11.845182	532.899324	11.999181
12.546872	534.218555	12.004199
12.119391	538.945817	12.009216
11.916176	529.181568	12.014234
12.196928	530.602981	12.019251
11.807876	532.334703	12.024269
12.189043	526.227774	12.029287
12.095269	531.812905	12.034304
11.836748	540.881591	12.039322
12.394672	536.719867	12.044339
12.241945	548.784623	12.049357
12.015534	530.590308	12.054375
12.268416	538.324784	12.059392
12.302006	546.469962	12.064410
12.329891	532.610814	12.069427
11.961875	536.147991	12.074445
12.270324	538.543298	12.079463
12.152030	556.378362	12.084480
12.397597	562.587387	12.089498
12.387347	552.398085	12.094515
12.141494	550.411452	12.099533
12.195410	539.890687	12.104551
12.441347	541.707013	12.109568
12.451432	546.039401	12.114586
12.384231	538.497952	12.119603
11.982416	549.031222	12.124621
12.352222	545.933257	12.129639
12.706276	560.157660	12.134656
12.430681	548.005340	12.139674
12.498939	534.430038	12.144691
12.291280	536.347852	12.149709
12.254685	531.277949	12.154727
12.394391	530.280358	12.159744
12.210528	530.460879	12.164762
12.433482	541.402268	12.169779
12.157299	554.245297	12.174797
12.542014	551.862139	12.179815
12.595936	561.283797	12.184832
12.431267	564.946353	12.189850
12.495275	558.448848	12.194867
12.306665	566.938685	12.199885
12.767071	549.477022	12.204903
12.836780	556.687937	12.209920
12.476264	549.019473	12.214938
12.297161	546.777315	12.219955
12.329353	556.561207	12.224973
12.459436	555.778776	12.229991
12.930784	553.661964	12.235008
12.533428	565.736928	12.240026
12.672236	554.607645	12.245043
12.597749	559.542980	12.250061
12.709236	560.758383	12.255079
12.815334	555.292820	12.260096
12.673841	561.191159	12.265114
12.791614	556.393305	12.270131
12.551116	562.095847	12.275149
12.634285	556.414803	12.280167
12.501224	564.222255	12.285184
12.277202	567.946999	12.290202
12.668819	565.004070	12.295219
12.223740	568.459927	12.300237
12.582131	562.864007	12.305255
12.682541	567.295609	12.310272
12.349352	566.427303	12.315290
12.482200	561.614747	12.320307
12.508869	572.264470	12.325325
12.781481	577.402160	12.330343
13.055367	586.994090	12.335360
12.616540	585.285060	12.340378
13.038786	578.075511	12.345395
12.939824	586.732392	12.350413
12.855197	584.843852	12.355431
13.033751	571.116011	12.360448
13.007448	573.437235	12.365466
12.978725	553.407122	12.370483
12.675885	552.366479	12.375501
12.990695	562.363795	12.380519
13.073707	561.870243	12.385536
12.695321	558.770981	12.390554
12.962657	560.727458	12.395571
13.334425	574.133245	12.400589
12.969499	570.591228	12.405607
12.863277	555.450805	12.410624
13.026836	562.208809	12.415642
13.024776	564.670496	12.420659
13.059661	576.918761	12.425677
13.217733	571.878417	12.430695
13.171599	559.872331	12.435712
13.193417	548.183328	12.440730
13.259458	548.341758	12.445747
12.779377	559.657237	12.450765
12.678620	550.761189	12.455783
13.189602	565.851286	12.460800
12.990037	572.583603	12.465818
12.942394	579.782861	12.470835
12.747194	577.028435	12.475853
13.307743	577.993113	12.480871
13.224594	580.727269	12.485888
13.297798	585.996008	12.490906
13.547131	578.998544	12.495923
13.354891	586.602040	12.500941
13.297410	581.572191	12.505959
13.294048	578.344687	12.510976
13.118856	575.763315	12.515994
13.186248	577.387178	12.521011
13.180632	579.969135	12.526029
13.398993	577.917832	12.531047
13.754290	586.111721	12.536064
13.038459	584.140706	12.541082
13.490856	578.178055	12.546099
13.503823	581.495471	12.551117
13.233642	578.218061	12.556135
13.177415	568.095807	12.561152
13.250316	580.846409	12.566170
13.900157	574.220001	12.571187
13.345893	572.945810	12.576205
13.479416	566.792280	12.581223
13.350811	563.218612	12.586240
13.218345	575.710322	12.591258
13.587743	578.820300	12.596275
13.082818	581.805390	12.601293
13.328286	583.217100	12.606311
13.280465	577.756546	12.611328
13.515256	581.619478	12.616346
13.343955	581.440461	12.621363
13.525726	581.355725	12.626381
13.343971	580.098192	12.631399
13.683321	569.038047	12.636416
13.157864	581.102347	12.641434
13.548963	571.444567	12.646451
13.604981	576.894878	12.651469
13.599080	580.387849	12.656487
13.994261	570.930562	12.661504
13.736195	574.516465	12.666522
13.596944	574.142783	12.671539
13.625517	576.960008	12.676557
13.423758	576.639981	12.681575
13.605545	581.000635	12.686592
13.090249	575.756853	12.691610
13.584090	582.819600	12.696627
13.504072	589.908483	12.701645
13.748049	603.796057	12.706663
14.096662	596.739235	12.711680
13.948976	605.634102	12.716698
14.215143	584.464633	12.721715
13.647113	577.869823	12.726733
13.179608	580.822734	12.731751
13.859742	580.173220	12.736768
13.875119	601.389535	12.741786
13.980612	599.076621	12.746803
13.901534	597.559185	12.751821
13.896655	590.883715	12.756839
13.736935	592.631796	12.761856
13.688908	600.412588	12.766874
13.816264	595.462357	12.771891
14.107678	591.110119	12.776909
14.044702	600.790120	12.781927
13.985603	603.319130	12.786944
13.743900	610.206069	12.791962
13.958987	599.868011	12.796979
13.795438	603.109157	12.801997
13.752092	608.585380	12.807015
14.358748	601.309065	12.812032
14.018796	606.694254	12.817050
14.030192	603.612323	12.822067
13.944140	605.957619	12.827085
14.170780	601.738931	12.832103
14.116527	594.531904	12.837120
14.158246	606.960939	12.842138
14.369755	607.472031	12.847155
14.534979	600.536119	12.852173
14.159593	583.627752	12.857191
14.002751	567.765823	12.862208
14.016818	572.289673	12.867226
13.992132	580.939763	12.872243
14.329866	590.687254	12.877261
14.182545	595.994875	12.882279
14.547510	590.979711	12.887296
14.313850	584.083482	12.892314
14.023999	573.415301	12.897331
14.495024	575.306950	12.902349
13.891988	578.971631	12.907367
14.388252	582.206656	12.912384
14.373549	597.919628	12.917402
14.369184	590.944090	12.922419
14.206033	592.462832	12.927437
14.304232	588.432336	12.932455
14.487592	591.049533	12.937472
14.094597	604.813466	12.942490
14.287036	595.589724	12.947507
14.166086	599.091121	12.952525
14.263955	600.668997	12.957543
14.239752	601.085270	12.962560
13.681695	600.768733	12.967578
14.121858	599.297197	12.972595
14.168937	601.211811	12.977613
14.302421	601.503159	12.982631
14.254067	602.915496	12.987648
14.364623	622.463029	12.992666
14.560171	621.299304	12.997683
14.787007	619.817425	13.002701
14.692919	618.694182	13.007719
14.712850	610.343041	13.012736
14.629584	596.494368	13.017754
14.298064	585.430347	13.022771
14.673453	597.664367	13.027789
14.641195	606.134634	13.032807
14.995783	599.284289	13.037824
14.348465	598.050700	13.042842
14.672267	585.330621	13.047859
14.744176	584.420823	13.052877
14.600515	588.493659	13.057895
14.613365	589.114413	13.062912
14.953746	607.941629	13.067930
14.900110	599.639288	13.072947
14.765022	590.082407	13.077965
14.694552	595.793418	13.082983
15.035195	589.162696	13.088000
14.840399	589.623357	13.093018
14.772007	586.759354	13.098035
15.234689	585.490770	13.103053
14.952380	583.186567	13.108071
14.734893	584.028521	13.113088
14.671175	587.809397	13.118106
14.482803	586.039211	13.123123
14.900014	589.338900	13.128141
14.614682	590.657809	13.133159
14.500138	583.495808	13.138176
14.723771	593.890896	13.143194
14.925738	618.438336	13.148211
15.266110	614.293720	13.153229
14.965491	615.947819	13.158247
15.142501	591.313784	13.163264
14.611687	591.697024	13.168282
14.995921	596.756005	13.173299
15.110040	603.721808	13.178317
14.915532	612.684665	13.183335
15.257498	602.454328	13.188352
14.894796	603.037670	13.193370
15.018254	611.338856	13.198387
15.169150	614.139769	13.203405
14.755969	613.791762	13.208423
15.269634	610.619179	13.213440
15.322548	619.334389	13.218458
15.146511	611.805021	13.223475
15.342402	613.952853	13.228493
15.030910	615.161142	13.233511
15.393254	618.430555	13.238528
15.298311	607.906048	13.243546
14.906900	603.943238	13.248563
15.101280	600.399144	13.253581
15.196302	605.333981	13.258599
15.692531	605.116864	13.263616
15.249632	606.535483	13.268634
15.109860	604.555685	13.273651
15.579436	609.124582	13.278669
15.185159	600.723538	13.283687
15.043764	600.563584	13.288704
15.160373	610.781536	13.293722
15.037236	611.689753	13.298739
15.195608	615.455905	13.303757
15.107523	610.184673	13.308775
15.188052	606.110644	13.313792
15.203840	603.557875	13.318810
15.207101	612.484047	13.323827
15.273946	601.529630	13.328845
15.407133	607.378958	13.333863
15.355837	600.319461	13.338880
15.590086	605.645786	13.343898
15.170165	607.047215	13.348915
15.329721	616.840762	13.353933
15.593128	635.772879	13.358951
15.815235	635.393292	13.363968
15.815443	635.535460	13.368986
15.623834	613.767777	13.374003
15.719895	602.282568	13.379021
15.668953	604.902348	13.384039
15.872489	595.468907	13.389056
16.023026	600.731144	13.394074
15.474142	609.173976	13.399091
15.851306	601.322707	13.404109
15.700580	600.456466	13.409127
15.858708	602.995959	13.414144
15.705360	603.706829	13.419162
15.518829	608.563494	13.424179
15.654650	602.442638	13.429197
15.660486	600.602892	13.434215
15.626062	608.044054	13.439232
15.673194	600.780474	13.444250
15.587791	608.843820	13.449267
15.836130	596.972004	13.454285
15.460753	603.350399	13.459303
15.868071	618.130962	13.464320
16.274195	627.538432	13.469338
15.990837	615.966049	13.474355
15.935741	602.532760	13.479373
15.618670	607.084683	13.484391
15.824772	603.659112	13.489408
16.154856	604.250169	13.494426
15.572050	609.499599	13.499443
16.242032	608.282903	13.504461
15.608895	611.575432	13.509479
15.781283	618.208384	13.514496
15.730214	622.616664	13.519514
16.028467	630.733020	13.524531
16.078580	623.579953	13.529549
16.208096	631.801412	13.534567
16.115031	631.521256	13.539584
16.223015	627.193084	13.544602
16.111801	635.255206	13.549619
16.295335	621.330444	13.554637
16.239454	639.096217	13.559655
16.325500	623.152675	13.564672
15.929949	613.645208	13.569690
16.125939	626.181382	13.574707
16.236447	629.202359	13.579725
16.242831	639.142143	13.584743
16.053388	635.799385	13.589760
16.241888	636.219411	13.594778
16.119533	639.932848	13.599795
16.459794	636.757874	13.604813
16.439015	638.529407	13.609831
16.131558	634.419229	13.614848
16.041010	638.146689	13.619866
15.860916	642.988127	13.624883
16.200526	629.944940	13.629901
16.250745	642.105682	13.634919
16.272424	629.351349	13.639936
16.487355	633.459694	13.644954
16.402895	636.902304	13.649971
16.689029	634.809065	13.654989
16.216270	632.302940	13.660007
16.432437	631.186978	13.665024
16.307495	641.373300	13.670042
16.322880	629.854188	13.675059
16.827562	634.234220	13.680077
16.410549	634.895843	13.685095
16.440368	636.464521	13.690112
16.552182	633.357295	13.695130
16.527122	631.240000	13.700147
16.776695	638.251889	13.705165
16.549150	624.638880	13.710183
16.696046	628.396307	13.715200
16.486840	624.349386	13.720218
16.330150	632.357230	13.725235
16.865832	624.724568	13.730253
16.822292	633.527801	13.735271
16.591630	635.651786	13.740288
16.740037	626.903793	13.745306
16.847559	635.248574	13.750323
16.610228	628.959590	13.755341
16.612513	643.035639	13.760359
16.362946	636.132572	13.765376
16.638935	631.853346	13.770394
16.426043	645.682761	13.775411
16.985583	656.174229	13.780429
16.948185	656.628119	13.785447
16.648332	660.949266	13.790464
16.974803	652.331607	13.795482
17.054033	662.040064	13.800499
16.968719	655.282615	13.805517
17.062357	653.376358	13.810535
16.694632	647.360126	13.815552
16.819486	645.086517	13.820570
16.951920	657.825356	13.825587
17.082629	667.272550	13.830605
17.007053	656.934557	13.835623
17.020424	667.461751	13.840640
17.146184	655.835371	13.845658
16.894303	662.653944	13.850675
17.031296	656.832462	13.855693
17.299324	660.785181	13.860711
17.009419	648.914269	13.865728
17.081853	642.581071	13.870746
16.705967	660.102632	13.875763
16.902578	660.205979	13.880781
16.813836	654.491558	13.885799
16.843712	651.505765	13.890816
17.319654	656.812950	13.895834
17.082222	658.498714	13.900851
17.346275	656.022930	13.905869
17.007861	657.950206	13.910887
17.306579	664.248103	13.915904
17.444763	650.717416	13.920922
17.176420	657.895779	13.925939
17.587324	654.159135	13.930957
17.154542	652.053450	13.935975
16.944711	654.379881	13.940992
17.467308	655.402815	13.946010
17.398996	657.042859	13.951027
17.742155	653.313102	13.956045
17.618315	651.453093	13.961063
17.009694	644.407521	13.966080
17.423291	639.463811	13.971098
17.294570	650.426703	13.976115
17.411337	647.636747	13.981133
17.543294	640.349654	13.986151
17.104221	641.549938	13.991168
17.592872	647.236884	13.996186
17.227996	642.966143	14.001203
17.479750	655.932846	14.006221
17.692349	665.813698	14.011239
17.412378	662.833937	14.016256
18.461099	662.116301	14.021274
17.839198	657.468849	14.026291
17.746258	643.111136	14.031309
17.623975	643.840877	14.036327
17.543414	652.547895	14.041344
17.967621	644.140028	14.046362
17.538253	648.194052	14.051379
17.753337	641.698265	14.056397
17.821508	645.976183	14.061415
17.727916	638.191825	14.066432
18.181929	644.004577	14.071450
17.710869	644.823567	14.076467
17.959521	651.317927	14.081485
17.859961	649.224777	14.086503
17.983065	645.772392	14.091520
17.911240	644.436023	14.096538
17.883641	642.493547	14.101555
17.715724	638.619696	14.106573
18.064027	650.240563	14.111591
17.544424	642.242904	14.116608
17.972758	643.225543	14.121626
17.632526	651.896824	14.126643
17.587788	644.797247	14.131661
17.908616	640.262576	14.136679
17.699425	644.811606	14.141696
18.003489	650.193705	14.146714
17.766925	660.938649	14.151731
17.917506	670.925044	14.156749
18.235630	669.850855	14.161767
17.810288	678.338617	14.166784
18.266485	672.542614	14.171802
18.198209	676.044755	14.176819
18.346483	676.598207	14.181837
18.491685	672.068989	14.186855
18.182599	663.558534	14.191872
18.204406	643.904559	14.196890
17.918498	647.365963	14.201907
18.239272	664.463919	14.206925
18.410504	669.660158	14.211943
18.155924	678.010594	14.216960
18.686948	662.759034	14.221978
18.198490	654.977458	14.226995
17.898329	653.217114	14.232013
18.137894	661.188883	14.237031
17.982537	666.695879	14.242048
18.185997	663.926601	14.247066
18.221965	670.704205	14.252083
18.132190	675.813752	14.257101
18.335093	671.971397	14.262119
18.125081	676.805201	14.267136
18.589221	667.595872	14.272154
18.321738	670.275140	14.277171
18.272115	674.246999	14.282189
18.524217	668.173000	14.287207
18.388311	675.015679	14.292224
18.601693	665.035714	14.297242
18.450107	678.236538	14.302259
18.371196	681.251097	14.307277
19.070849	684.420185	14.312295
18.682379	686.043959	14.317312
18.682878	669.144904	14.322330
18.915496	673.757389	14.327347
18.760062	673.154508	14.332365
18.706971	660.831009	14.337383
18.419632	674.122022	14.342400
18.755946	664.642538	14.347418
18.689492	662.190381	14.352435
18.572425	662.199221	14.357453
18.759447	667.575118	14.362471
18.948487	686.974705	14.367488
18.954467	676.936168	14.372506
18.901043	665.117418	14.377523
18.409430	667.861750	14.382541
18.970160	679.752565	14.387559
18.691113	688.939296	14.392576
19.234797	686.751437	14.397594
18.958557	699.824110	14.402611
18.902747	691.940560	14.407629
19.251201	685.778950	14.412647
19.034687	681.466310	14.417664
18.896248	662.137256	14.422682
18.854046	669.710436	14.427699
18.970399	686.066719	14.432717
19.478058	694.246854	14.437735
18.921014	684.549167	14.442752
18.998041	667.428005	14.447770
19.155508	682.467313	14.452787
18.938888	684.859831	14.457805
19.232538	684.954589	14.462823
19.173985	690.643978	14.467840
19.034026	693.410789	14.472858
19.074665	692.633714	14.477875
19.157177	701.361786	14.482893
19.348714	696.067055	14.487911
19.055239	695.985034	14.492928
19.296076	705.863205	14.497946
19.541001	702.844154	14.502963
19.235150	700.123381	14.507981
19.200395	687.314568	14.512999
19.250093	702.500869	14.518016
19.394151	698.589121	14.523034
19.225479	701.762241	14.528051
19.255520	711.934362	14.533069
19.469659	707.511822	14.538087
19.307894	700.539466	14.543104
19.054366	702.665278	14.548122
19.430134	699.813921	14.553139
19.010516	691.643389	14.558157
19.330395	695.255659	14.563175
19.353047	699.543097	14.568192
18.917950	694.394255	14.573210
19.543575	715.550224	14.578227
19.489974	721.239985	14.583245
19.847441	729.837114	14.588263
19.829141	729.608352	14.593280
19.549404	720.202501	14.598298
20.223135	728.974413	14.603315
19.400490	717.841629	14.608333
19.291483	708.828751	14.613351
19.533817	723.463517	14.618368
19.529492	718.501983	14.623386
19.634914	724.922459	14.628403
19.661380	730.774940	14.633421
19.755361	724.201146	14.638439
19.382051	727.753808	14.643456
19.452545	728.352818	14.648474
19.543563	721.959428	14.653491
19.461092	721.745622	14.658509
20.019168	730.321343	14.663527
20.185425	740.025281	14.668544
20.285891	731.288711	14.673562
20.168531	727.428905	14.678579
19.964408	724.932215	14.683597
20.000458	722.329617	14.688615
19.841178	724.679577	14.693632
20.153150	717.925601	14.698650
20.462830	718.477131	14.703667
20.172918	716.825312	14.708685
20.165757	715.044001	14.713703
20.125496	710.896250	14.718720
19.889702	726.855007	14.723738
20.298165	715.494353	14.728755
20.022695	722.928243	14.733773
20.070823	711.123348	14.738791
20.131404	716.046996	14.743808
20.341817	718.390065	14.748826
20.226019	720.783609	14.753843
19.985819	719.633374	14.758861
20.365449	715.562935	14.763879
20.393762	715.104419	14.768896
20.186340	715.691971	14.773914
20.249417	715.875695	14.778931
20.236190	716.581476	14.783949
20.477556	714.166523	14.788967
20.135249	725.495921	14.793984
20.392835	729.474007	14.799002
20.742862	734.181630	14.804019
20.435143	728.540842	14.809037
20.103924	721.155614	14.814055
19.907647	730.714470	14.819072
20.298224	745.494779	14.824090
20.669779	737.697912	14.829107
20.643825	741.882786	14.834125
21.014876	739.001103	14.839143
20.493824	743.082144	14.844160
20.478596	750.011954	14.849178
20.682752	739.328387	14.854195
20.586871	741.234802	14.859213
20.714402	726.448791	14.864231
20.716182	730.915276	14.869248
20.665466	732.072124	14.874266
21.006201	739.366586	14.879283
20.740143	740.519725	14.884301
20.849968	736.121143	14.889319
20.720336	733.934147	14.894336
20.533064	735.755306	14.899354
20.770346	739.051753	14.904371
20.506997	742.325594	14.909389
20.727301	736.067474	14.914407
21.119096	747.089905	14.919424
20.763805	740.896388	14.924442
20.906206	738.380108	14.929459
20.958710	740.696576	14.934477
20.840796	732.727625	14.939495
20.716922	736.502750	14.944512
20.873119	742.455402	14.949530
20.920067	732.758058	14.954547
20.345467	734.646504	14.959565
20.909226	744.990491	14.964583
21.202778	750.347202	14.969600
21.156321	769.154424	14.974618
20.985746	761.799660	14.979635
21.118418	766.840514	14.984653
21.377248	762.071599	14.989671
21.242725	752.289731	14.994688
21.235737	749.289552	14.999706
21.221931	752.308305	15.004723
21.269311	764.782196	15.009741
21.404955	763.725226	15.014759
21.254733	751.550410	15.019776
21.153801	747.542611	15.024794
21.361181	757.993649	15.029811
21.203283	767.665852	15.034829
21.187707	771.930508	15.039847
21.280430	760.399674	15.044864
21.054309	764.574789	15.049882
21.261421	761.863942	15.054899
21.608030	768.081514	15.059917
21.386463	763.439782	15.064935
21.474378	765.579138	15.069952
21.163676	770.203278	15.074970
21.496745	755.911131	15.079987
21.418889	755.568614	15.085005
21.249952	754.670342	15.090023
21.508549	759.993083	15.095040
21.368340	765.849950	15.100058
21.532595	766.617678	15.105075
21.762109	782.960837	15.110093
21.860610	785.024037	15.115111
21.783147	772.593074	15.120128
21.589152	770.392322	15.125146
21.769149	780.032202	15.130163
22.149226	784.868717	15.135181
22.023041	768.838127	15.140199
21.787524	763.302687	15.145216
21.502849	762.013757	15.150234
21.861529	753.134816	15.155251
21.478204	769.142454	15.160269
21.689404	773.806546	15.165287
21.993613	784.247473	15.170304
22.090085	785.874416	15.175322
22.333879	783.137413	15.180339
21.847138	778.006542	15.185357
22.198746	774.417870	15.190375
22.031347	756.182023	15.195392
21.409433	762.231640	15.200410
21.831715	767.289495	15.205427
22.220269	786.099899	15.210445
21.926595	794.134446	15.215463
22.348077	780.134708	15.220480
22.289920	789.053436	15.225498
22.417863	791.363718	15.230515
22.240458	797.070071	15.235533
22.250106	783.547167	15.240551
22.334209	786.037140	15.245568
22.124922	788.805999	15.250586
22.496849	780.929918	15.255603
22.311863	779.126080	15.260621
22.433915	764.661396	15.265639
22.087173	764.666932	15.270656
22.181081	781.671488	15.275674
22.508383	788.252485	15.280691
22.185926	791.847525	15.285709
22.452058	788.628105	15.290727
22.646251	784.902120	15.295744
22.486501	787.640730	15.300762
22.414699	783.552905	15.305779
21.940196	782.706804	15.310797
22.269693	785.961615	15.315815
22.364045	785.851593	15.320832
22.556597	787.803949	15.325850
22.659007	785.062405	15.330867
22.783738	785.216237	15.335885
22.746948	779.639617	15.340903
22.852498	783.794854	15.345920
22.629205	789.746192	15.350938
22.643014	782.530956	15.355955
22.361985	775.715710	15.360973
22.378457	783.620946	15.365991
22.661821	787.654225	15.371008
22.291970	781.807574	15.376026
22.616691	794.853251	15.381043
22.600010	811.487196	15.386061
22.647943	809.076701	15.391079
23.242037	808.110342	15.396096
23.090373	805.780534	15.401114
23.104539	803.611841	15.406131
23.186017	815.026240	15.411149
22.942097	822.860052	15.416167
23.212631	806.906244	15.421184
22.661374	805.661060	15.426202
22.727080	795.957421	15.431219
23.130764	799.189321	15.436237
23.184808	803.164519	15.441255
23.150273	797.364301	15.446272
23.068333	808.316409	15.451290
23.035468	803.976867	15.456307
23.012576	808.470293	15.461325
23.211320	814.450964	15.466343
23.705526	807.755353	15.471360
23.400133	808.320156	15.476378
23.361157	811.164356	15.481395
23.344734	810.166814	15.486413
23.237701	811.408974	15.491431
23.565191	811.003273	15.496448
23.221148	811.065839	15.501466
23.164485	800.002998	15.506483
23.485745	804.566595	15.511501
22.987499	804.571234	15.516519
23.199581	807.902970	15.521536
23.242179	811.500555	15.526554
23.319317	799.641580	15.531571
23.144029	799.902963	15.536589
23.052736	803.476656	15.541607
23.211818	796.121222	15.546624
23.145155	808.988425	15.551642
23.509405	817.535664	15.556659
23.835943	825.119118	15.561677
23.558951	828.146428	15.566695
23.797282	824.271005	15.571712
23.703760	827.391157	15.576730
23.738923	824.535945	15.581747
23.902383	828.267844	15.586765
23.493750	822.911435	15.591783
24.058961	821.971511	15.596800
23.860868	832.201959	15.601818
23.829429	829.851846	15.606835
23.835848	825.532957	15.611853
23.734193	824.212928	15.616871
24.019316	820.157719	15.621888
24.161456	833.205711	15.626906
23.952858	818.487476	15.631923
24.302789	827.181966	15.636941
23.693569	817.977063	15.641959
23.864552	820.045981	15.646976
23.685911	831.612909	15.651994
23.921617	829.320524	15.657011
24.033069	819.905739	15.662029
23.478617	824.134844	15.667047
23.519530	819.911421	15.672064
23.728269	831.022489	15.677082
24.570893	828.155218	15.682099
24.155833	825.830441	15.687117
24.056067	833.620705	15.692135
24.360933	817.213190	15.697152
24.292818	824.777352	15.702170
24.231354	832.321914	15.707187
24.143031	825.488514	15.712205
24.278109	846.681407	15.717223
24.338859	851.033442	15.722240
24.317983	857.899278	15.727258
24.588619	850.413934	15.732275
24.395203	852.599493	15.737293
24.503420	851.915940	15.742311
24.577671	850.976213	15.747328
24.445956	862.796799	15.752346
24.560703	855.092789	15.757363
24.876752	854.148060	15.762381
24.709266	848.491880	15.767399
24.541340	839.830792	15.772416
24.412552	843.545737	15.777434
24.960418	849.735529	15.782451
24.841934	847.574622	15.787469
24.534450	833.904984	15.792487
24.692342	841.763211	15.797504
24.882834	858.334161	15.802522
24.715904	854.230575	15.807539
24.954035	847.627741	15.812557
24.829003	847.086744	15.817575
24.704913	832.987150	15.822592
24.622754	847.303735	15.827610
24.831802	846.614903	15.832627
24.772987	856.370356	15.837645
24.955352	851.892015	15.842663
24.719908	851.348436	15.847680
24.664669	855.526380	15.852698
24.758858	856.302959	15.857715
24.867506	851.774624	15.862733
24.994396	853.928404	15.867751
25.074246	845.302659	15.872768
24.873920	853.168636	15.877786
25.035636	845.814711	15.882803
25.217172	844.828480	15.887821
24.774188	851.924832	15.892839
24.766100	844.365177	15.897856
24.883290	860.417189	15.902874
25.256234	873.356921	15.907891
25.505056	870.989527	15.912909
24.983356	882.418819	15.917927
25.204417	881.247702	15.922944
25.045897	879.246169	15.927962
25.242826	882.074153	15.932979
25.144237	884.089297	15.937997
25.197437	883.278245	15.943015
25.577740	878.206515	15.948032
25.427445	876.671711	15.953050
25.230511	880.035759	15.958067
25.486386	874.485837	15.963085
25.524867	874.426008	15.968103
25.568694	874.246796	15.973120
25.373006	877.638983	15.978138
25.317023	881.985554	15.983155
25.876771	898.751298	15.988173
25.630670	905.732399	15.993191
26.019543	897.732986	15.998208
25.828057	885.338135	16.003226
25.732739	876.650044	16.008243
25.598076	873.461148	16.013261
25.584536	885.973177	16.018279
25.873206	889.319019	16.023296
25.533987	897.869407	16.028314
25.906678	909.758862	16.033331
26.010748	892.372747	16.038349
25.878050	907.277653	16.043367
26.067559	892.615468	16.048384
26.088379	900.957034	16.053402
25.930992	904.262572	16.058419
26.231065	895.760169	16.063437
25.916135	901.988131	16.068455
26.075547	904.512108	16.073472
26.367107	901.884886	16.078490
26.168993	897.296314	16.083507
26.312231	905.490451	16.088525
25.972880	905.300676	16.093543
26.128562	896.395428	16.098560
26.115499	896.851988	16.103578
26.002159	894.078831	16.108595
25.933869	891.849766	16.113613
26.074937	899.661205	16.118631
26.403668	898.819881	16.123648
26.329363	891.338094	16.128666
26.018530	906.683897	16.133683
26.475724	891.747081	16.138701
26.271920	905.676794	16.143719
26.077109	894.647784	16.148736
26.127725	903.019848	16.153754
26.088677	917.785640	16.158771
26.594327	918.665343	16.163789
26.535835	923.621766	16.168807
26.676064	923.125027	16.173824
26.900215	911.528619	16.178842
26.614919	921.862932	16.183859
27.051906	916.313318	16.188877
26.547948	908.516070	16.193895
26.676987	898.794400	16.198912
26.964217	910.550769	16.203930
26.655238	898.342285	16.208947
26.702459	893.979614	16.213965
26.412136	913.208085	16.218983
26.935742	918.651165	16.224000
26.847047	916.529015	16.229018
26.793972	920.141287	16.234035
27.121814	916.180156	16.239053
27.191956	912.687665	16.244071
26.981259	909.763310	16.249088
26.973234	900.191889	16.254106
26.828591	920.103697	16.259123
27.184104	909.974848	16.264141
26.785944	912.523440	16.269159
26.931375	911.010133	16.274176
27.259123	908.628090	16.279194
26.962143	902.822079	16.284211
27.097894	904.003573	16.289229
27.093105	912.036799	16.294247
26.825259	914.448463	16.299264
27.140256	908.558437	16.304282
26.930521	915.510293	16.309299
27.090029	913.261221	16.314317
26.915899	917.827358	16.319335
26.994579	934.124002	16.324352
27.565386	936.696394	16.329370
27.474047	944.805384	16.334387
27.378824	941.879618	16.339405
27.553993	940.485789	16.344423
27.735574	947.096889	16.349440
27.822290	932.380824	16.354458
27.386560	941.727108	16.359475
27.761043	939.413695	16.364493
27.469217	941.600603	16.369511
27.767629	944.238966	16.374528
27.838428	949.969233	16.379546
27.387332	942.688785	16.384563
27.818958	940.954864	16.389581
27.960887	941.875899	16.394599
27.727294	936.445979	16.399616
27.859954	936.245364	16.404634
27.790670	933.286959	16.409651
27.922319	943.557363	16.414669
27.756553	940.079521	16.419687
28.149868	939.405446	16.424704
28.082560	931.218966	16.429722
27.853328	929.716518	16.434739
27.911651	924.816588	16.439757
28.041730	934.591991	16.444775
28.272054	931.684365	16.449792
28.087810	923.159392	16.454810
27.899252	922.127750	16.459827
28.170270	925.885956	16.464845
28.142179	924.686409	16.469863
27.995893	927.931456	16.474880
28.130217	919.941112	16.479898
27.834299	932.158611	16.484915
28.027339	922.366489	16.489933
27.881064	926.231193	16.494951
27.864061	930.582346	16.499968
28.259359	926.263994	16.504986
28.298986	931.812416	16.510003
28.062726	930.902053	16.515021
28.185679	940.780604	16.520039
28.158880	958.695860	16.525056
28.690047	957.320244	16.530074
28.239031	960.770475	16.535091
28.361103	954.742698	16.540109
28.869355	961.588677	16.545127
28.467909	960.809599	16.550144
28.483400	952.642073	16.555162
28.632533	964.518590	16.560179
28.906069	954.566667	16.565197
28.895084	957.460587	16.570215
28.680098	957.998614	16.575232
28.990618	954.746221	16.580250
28.528788	969.152164	16.585267
28.782484	954.298984	16.590285
28.941484	950.108725	16.595303
28.757340	945.421767	16.600320
28.806022	953.533165	16.605338
28.762355	958.852485	16.610355
28.778122	950.426656	16.615373
28.711738	951.534148	16.620391
28.644547	953.227578	16.625408
28.775751	945.336554	16.630426
28.808839	949.617216	16.635443
28.840307	943.901679	16.640461
29.178943	957.912871	16.645479
29.135296	975.336072	16.650496
29.342360	977.820676	16.655514
29.041831	973.873820	16.660531
29.212441	974.760187	16.665549
29.287831	970.980998	16.670567
29.222172	970.351428	16.675584
29.817714	970.896576	16.680602
29.663652	971.711906	16.685619
29.382106	954.167930	16.690637
29.585558	952.228492	16.695655
29.426987	954.608682	16.700672
29.275872	936.273866	16.705690
29.218824	951.809964	16.710707
29.693622	965.447842	16.715725
29.559681	964.831547	16.720743
29.672488	959.593463	16.725760
29.746348	951.427295	16.730778
29.389736	956.147671	16.735795
29.651600	958.772798	16.740813
30.015879	968.575187	16.745831
29.843593	959.010064	16.750848
29.626765	947.489404	16.755866
29.821752	941.136186	16.760883
29.870810	950.912811	16.765901
29.873200	941.045163	16.770919
29.589974	958.132834	16.775936
29.968923	958.478422	16.780954
30.201302	967.465675	16.785971
29.930473	971.995480	16.790989
29.831147	964.907550	16.796007
29.499761	969.719025	16.801024
29.759614	965.174280	16.806042
29.992985	980.161548	16.811059
30.516338	977.224683	16.816077
29.997663	968.402712	16.821095
29.829258	965.727634	16.826112
30.119225	970.631489	16.831130
30.265861	980.706531	16.836147
29.960628	982.927552	16.841165
30.306818	977.514207	16.846183
30.369540	980.477027	16.851200
30.341927	978.075079	16.856218
30.308262	979.573597	16.861235
30.292427	979.599532	16.866253
30.614874	974.244842	16.871271
30.311717	978.905981	16.876288
29.922455	972.113687	16.881306
30.074818	972.553092	16.886323
30.421155	993.257678	16.891341
30.503880	1000.075715	16.896359
30.470122	1007.941353	16.901376
31.073371	998.891859	16.906394
30.791406	999.698843	16.911411
30.444610	1003.910145	16.916429
30.868356	999.281561	16.921447
30.471434	1006.486886	16.926464
30.879559	1000.943203	16.931482
30.717275	998.091521	16.936499
30.629862	1005.837307	16.941517
30.822094	996.635802	16.946535
30.601381	1000.418759	16.951552
30.679387	1000.977561	16.956570
30.679772	1002.448791	16.961587
30.808814	994.323855	16.966605
30.905656	995.077562	16.971623
30.503864	997.529134	16.976640
30.869407	1002.385447	16.981658
31.122346	1017.739578	16.986675
31.170529	1021.819342	16.991693
31.624773	1019.354527	16.996711
31.482551	1023.619358	17.001728
31.321481	998.494219	17.006746
31.449325	993.782355	17.011763
31.039509	987.317067	17.016781
31.242791	992.342760	17.021799
31.103232	1011.251911	17.026816
31.764801	1017.925289	17.031834
31.230857	1010.840803	17.036851
31.396075	1024.370946	17.041869
31.673878	1014.504889	17.046887
31.480501	1022.365470	17.051904
31.637941	1022.776872	17.056922
31.852513	1018.999427	17.061939
31.366045	997.130820	17.066957
31.585423	1009.057943	17.071975
31.314800	1012.313753	17.076992
31.439388	1016.047410	17.082010
31.637553	1014.140336	17.087027
31.647640	1027.091465	17.092045
31.827626	1017.927407	17.097063
31.710055	1025.870317	17.102080
31.612237	1019.847037	17.107098
31.649697	1019.579904	17.112115
31.602866	1021.233358	17.117133
31.624785	1006.199223	17.122151
31.901474	1023.403693	17.127168
32.039912	1024.989856	17.132186
32.223845	1032.675371	17.137203
32.131121	1026.916197	17.142221
32.162606	1016.546062	17.147239
32.048545	1021.563684	17.152256
31.960329	1028.610032	17.157274
32.048745	1036.384984	17.162291
32.201816	1037.828966	17.167309
32.479038	1044.010505	17.172327
32.071531	1038.354236	17.177344
32.213365	1035.434473	17.182362
32.525917	1041.883380	17.187379
32.143871	1041.391233	17.192397
32.352462	1036.458512	17.197415
32.300095	1040.591150	17.202432
32.040494	1039.597246	17.207450
32.370167	1038.784499	17.212467
32.102205	1036.889254	17.217485
32.336691	1031.195185	17.222503
32.308057	1035.925840	17.227520
32.664427	1050.696360	17.232538
32.708384	1056.869287	17.237555
32.749823	1059.034883	17.242573
32.998575	1049.286997	17.247591
32.980553	1052.945856	17.252608
32.821246	1041.749449	17.257626
32.760926	1026.802138	17.262643
32.613462	1034.699610	17.267661
32.625235	1027.057446	17.272679
32.447659	1048.490963	17.277696
32.667866	1061.558504	17.282714
33.031669	1068.899696	17.287731
33.025351	1062.806526	17.292749
33.174187	1058.696266	17.297767
33.326584	1064.356373	17.302784
33.468778	1066.798585	17.307802
33.499448	1060.856766	17.312819
33.254057	1061.637225	17.317837
33.434674	1048.965673	17.322855
33.285881	1036.843937	17.327872
33.051780	1025.148920	17.332890
33.013947	1035.037227	17.337907
33.037991	1051.745785	17.342925
33.203715	1055.412407	17.347943
33.317659	1062.822527	17.352960
33.257044	1057.262349	17.357978
33.221990	1057.991838	17.362995
32.940495	1057.762166	17.368013
33.281706	1055.752662	17.373031
33.337681	1055.529706	17.378048
33.393221	1069.057183	17.383066
33.572180	1073.105070	17.388083
33.649669	1077.163068	17.393101
34.162239	1077.649521	17.398119
34.344394	1083.401162	17.403136
34.110290	1067.078692	17.408154
33.869547	1062.731374	17.413171
33.834543	1057.000032	17.418189
33.645394	1052.863064	17.423207
33.764564	1051.876911	17.428224
33.796738	1057.544719	17.433242
34.130898	1060.951962	17.438259
33.842639	1058.356160	17.443277
34.144534	1065.791457	17.448295
34.031514	1070.189257	17.453312
34.138187	1075.845916	17.458330
34.065759	1074.134424	17.463347
34.081373	1086.854773	17.468365
34.406265	1078.443828	17.473383
34.222560	1080.904574	17.478400
34.284363	1076.480778	17.483418
34.209483	1083.114718	17.488435
33.979293	1080.338829	17.493453
34.298204	1075.402395	17.498471
34.398479	1083.410046	17.503488
34.635120	1077.806939	17.508506
34.588607	1086.160935	17.513523
34.324831	1089.890416	17.518541
34.417922	1069.990640	17.523559
34.375349	1082.590309	17.528576
34.175578	1086.245414	17.533594
34.544659	1066.437733	17.538611
34.195813	1080.129028	17.543629
34.349541	1071.162982	17.548647
34.322468	1088.056416	17.553664
34.311606	1098.744999	17.558682
35.049208	1104.859385	17.563699
34.867791	1110.716512	17.568717
35.201102	1093.223317	17.573735
35.263132	1099.473187	17.578752
35.132303	1091.900272	17.583770
35.462809	1084.404903	17.588787
35.196086	1068.970877	17.593805
35.130295	1065.984310	17.598823
35.000866	1063.473227	17.603840
34.789676	1060.004453	17.608858
35.381673	1055.414527	17.613875
35.239531	1058.914811	17.618893
34.969721	1056.620669	17.623911
35.303977	1055.416230	17.628928
35.011079	1054.578622	17.633946
35.155075	1061.955026	17.638963
35.310505	1084.255865	17.643981
35.538033	1087.673291	17.648999
35.508843	1090.053731	17.654016
35.399903	1098.005877	17.659034
35.731191	1085.814056	17.664051
35.489881	1097.008893	17.669069
35.786447	1097.995668	17.674087
35.654974	1093.313721	17.679104
35.662303	1076.601274	17.684122
35.488439	1078.835987	17.689139
35.658677	1084.128198	17.694157
35.749879	1089.600028	17.699175
35.763144	1084.645699	17.704192
35.594023	1092.306243	17.709210
35.807413	1082.664582	17.714227
35.531779	1089.352238	17.719245
35.508964	1087.182149	17.724263
35.943340	1083.706864	17.729280
35.696804	1082.385214	17.734298
35.921763	1074.850635	17.739315
35.585253	1091.079585	17.744333
36.144762	1095.647519	17.749351
36.352390	1103.197653	17.754368
35.985798	1103.861573	17.759386
36.251470	1105.201485	17.764403
36.310062	1113.467228	17.769421
36.399527	1103.213415	17.774439
36.288842	1094.012406	17.779456
36.280901	1106.022913	17.784474
36.686761	1104.250329	17.789491
36.485334	1103.226711	17.794509
36.218719	1092.098035	17.799527
36.254069	1096.146480	17.804544
36.154813	1113.052682	17.809562
36.421765	1104.153693	17.814579
36.560372	1120.813829	17.819597
36.394331	1106.086697	17.824615
36.608731	1108.005557	17.829632
36.337943	1111.179921	17.834650
36.685134	1105.387637	17.839667
36.428636	1113.093366	17.844685
36.785672	1108.349028	17.849703
36.463568	1103.387235	17.854720
36.582610	1125.585895	17.859738
36.790674	1134.072561	17.864755
36.913738	1136.128592	17.869773
37.135378	1137.456901	17.874791
37.414554	1123.607188	17.879808
37.253906	1131.517915	17.884826
37.377001	1120.916798	17.889843
37.086607	1112.128596	17.894861
37.171176	1101.789770	17.899879
37.122803	1096.996427	17.904896
37.360368	1096.225306	17.909914
37.385448	1089.814337	17.914931
37.247290	1088.553478	17.919949
36.938491	1092.327421	17.924967
36.916886	1102.530792	17.929984
36.875740	1120.152949	17.935002
37.509985	1117.653590	17.940019
37.374963	1120.741303	17.945037
37.530952	1121.602936	17.950055
37.649534	1127.098592	17.955072
37.473036	1129.650276	17.960090
37.661739	1131.552921	17.965107
37.751407	1124.504882	17.970125
37.727433	1121.694445	17.975143
37.847432	1121.052630	17.980160
37.339387	1117.642840	17.985178
37.744015	1116.463357	17.990195
37.603447	1122.684974	17.995213
37.744783	1123.399038	18.000231
37.621291	1111.251400	18.005248
37.623624	1130.524198	18.010266
38.123437	1130.403727	18.015283
37.887701	1132.988055	18.020301
38.198975	1142.826104	18.025319
37.979595	1129.250272	18.030336
37.775096	1129.366500	18.035354
38.071258	1133.047368	18.040371
38.037047	1136.009339	18.045389
37.925649	1128.526099	18.050407
38.389469	1133.769715	18.055424
37.893130	1129.703276	18.060442
38.421290	1133.407932	18.065459
38.532502	1155.020544	18.070477
38.362555	1142.856165	18.075495
38.946642	1136.539222	18.080512
38.566101	1136.138945	18.085530
39.040423	1125.153692	18.090547
38.888654	1129.507532	18.095565
38.842447	1124.623273	18.100583
38.625941	1119.941225	18.105600
38.505094	1136.353797	18.110618
38.722323	1121.698222	18.115635
38.737600	1125.669686	18.120653
38.615957	1124.448608	18.125671
38.788419	1124.779575	18.130688
38.873295	1134.569676	18.135706
38.869807	1147.976686	18.140723
39.120452	1157.404322	18.145741
38.825548	1163.428289	18.150759
39.144034	1150.688156	18.155776
39.267673	1163.689100	18.160794
39.102944	1159.901594	18.165811
39.466586	1157.289166	18.170829
39.062278	1162.245842	18.175847
39.243233	1162.321473	18.180864
39.113241	1161.296651	18.185882
39.065939	1157.433798	18.190899
39.245428	1163.402046	18.195917
39.176568	1164.424532	18.200935
39.706337	1160.268885	18.205952
39.329948	1159.003374	18.210970
39.621650	1156.354828	18.215987
39.704170	1157.262880	18.221005
39.611827	1164.491070	18.226023
39.678519	1148.512792	18.231040
39.608704	1155.132145	18.236058
39.690856	1155.480035	18.241075
39.774604	1158.201224	18.246093
39.572961	1156.541039	18.251111
40.202846	1153.797521	18.256128
40.019652	1155.794033	18.261146
39.714255	1150.574740	18.266163
39.945794	1148.084579	18.271181
39.654800	1153.289411	18.276199
39.816168	1150.315212	18.281216
39.747046	1147.582717	18.286234
39.675906	1146.630827	18.291251
39.644594	1167.710771	18.296269
39.893640	1175.573761	18.301287
40.145411	1173.878258	18.306304
40.040357	1178.014145	18.311322
40.177027	1178.457337	18.316339
40.075030	1178.119989	18.321357
40.007452	1181.349299	18.326375
40.469841	1171.847844	18.331392
40.271490	1179.407761	18.336410
40.512152	1194.545602	18.341427
40.919015	1201.964371	18.346445
40.640753	1185.322717	18.351463
40.552863	1164.569736	18.356480
40.416117	1174.576476	18.361498
40.657203	1189.709912	18.366515
41.134155	1194.226981	18.371533
40.657820	1200.227461	18.376551
40.847501	1200.015827	18.381568
41.301680	1196.890381	18.386586
41.042190	1191.557569	18.391603
41.003873	1170.407404	18.396621
40.911359	1171.347195	18.401639
41.052080	1166.131584	18.406656
40.934862	1171.615120	18.411674
41.256361	1187.361995	18.416691
41.365220	1180.454056	18.421709
40.954415	1185.509450	18.426727
41.444177	1193.446367	18.431744
41.575851	1189.328678	18.436762
40.982176	1180.581206	18.441779
40.962938	1187.039446	18.446797
41.064834	1199.462143	18.451815
41.122746	1197.744409	18.456832
41.096027	1195.101733	18.461850
41.357667	1199.850120	18.466867
41.440442	1188.560373	18.471885
41.251170	1192.899969	18.476903
41.647734	1194.692616	18.481920
41.493426	1203.846790	18.486938
41.780439	1217.568348	18.491955
41.624707	1213.074236	18.496973
41.587867	1220.499557	18.501991
41.828003	1227.337692	18.507008
41.862867	1219.512479	18.512026
41.686934	1225.032134	18.517043
42.046607	1211.359560	18.522061
41.962085	1219.666380	18.527079
41.956900	1211.856858	18.532096
41.805907	1210.879210	18.537114
41.890842	1217.550523	18.542131
41.790016	1205.060876	18.547149
41.915976	1210.238418	18.552167
42.083575	1229.277679	18.557184
42.539968	1237.489429	18.562202
42.401890	1242.647711	18.567219
42.752644	1229.719498	18.572237
42.626918	1229.731739	18.577255
42.704703	1213.869664	18.582272
42.420440	1209.667303	18.587290
42.713528	1202.691054	18.592307
42.641654	1204.445915	18.597325
42.321334	1203.948265	18.602343
42.653724	1197.131649	18.607360
42.554491	1199.949284	18.612378
42.394533	1202.815163	18.617395
43.232649	1216.178150	18.622413
43.050264	1227.480250	18.627431
43.045852	1211.314472	18.632448
42.851133	1203.627674	18.637466
42.844488	1207.927979	18.642483
42.977930	1205.442241	18.647501
42.859005	1222.928973	18.652519
42.961406	1218.781872	18.657536
43.051578	1227.577476	18.662554
42.883185	1241.467374	18.667571
42.900287	1235.011604	18.672589
43.079863	1232.552868	18.677607
42.911022	1230.997871	18.682624
43.336635	1231.409362	18.687642
43.134447	1228.971715	18.692659
43.511283	1232.245950	18.697677
43.050674	1233.567949	18.702695
43.408161	1240.932710	18.707712
43.702205	1256.936953	18.712730
43.708808	1262.557496	18.717747
44.217464	1249.541704	18.722765
44.150090	1245.275861	18.727783
43.916354	1228.693714	18.732800
43.858262	1231.917527	18.737818
43.518024	1234.774288	18.742835
43.922219	1218.626275	18.747853
43.500363	1228.923168	18.752871
43.618701	1229.845372	18.757888
43.802788	1240.349019	18.762906
43.704333	1249.489248	18.767923
43.812117	1248.523472	18.772941
44.016905	1255.600539	18.777959
43.986013	1251.936122	18.782976
44.406349	1257.633429	18.787994
44.144072	1254.440781	18.793011
44.228728	1239.344458	18.798029
43.590688	1259.169112	18.803047
44.063074	1261.194876	18.808064
44.287442	1265.747885	18.813082
44.448793	1277.333255	18.818099
44.967037	1271.188971	18.823117
44.617879	1276.221194	18.828135
44.999015	1274.102693	18.833152
45.141821	1258.868377	18.838170
44.762808	1254.694684	18.843187
44.895034	1240.483772	18.848205
44.739436	1242.648951	18.853223
44.925681	1231.046376	18.858240
44.934775	1232.413038	18.863258
44.451633	1233.386806	18.868275
44.928194	1249.526172	18.873293
44.675616	1251.753078	18.878311
45.059518	1261.087848	18.883328
45.223313	1278.232164	18.888346
44.970907	1272.373750	18.893363
45.346849	1268.865189	18.898381
45.261914	1270.291912	18.903399
44.957880	1273.528898	18.908416
45.439690	1264.156847	18.913434
45.175036	1264.083827	18.918451
45.361400	1271.140724	18.923469
45.340772	1269.485198	18.928487
45.323753	1262.842156	18.933504
45.602245	1263.938627	18.938522
45.263452	1263.642848	18.943539
45.687686	1262.800260	18.948557
45.533524	1271.089111	18.953575
45.375116	1274.477178	18.958592
45.557915	1262.829089	18.963610
45.498156	1263.787083	18.968627
45.877506	1273.956458	18.973645
45.708288	1288.294559	18.978663
45.703981	1293.521651	18.983680
46.009706	1287.682624	18.988698
45.968358	1293.952840	18.993715
46.120949	1284.488835	18.998733
45.753951	1292.921206	19.003751
45.954039	1292.755091	19.008768
46.114258	1277.321421	19.013786
46.012682	1276.181652	19.018803
46.094431	1280.977568	19.023821
46.219667	1284.703310	19.028839
46.172610	1289.565045	19.033856
46.286682	1283.703817	19.038874
46.641771	1304.132181	19.043891
46.463377	1297.089473	19.048909
46.563221	1299.374565	19.053927
46.684034	1307.567118	19.058944
47.030494	1297.963918	19.063962
46.945871	1285.665615	19.068979
47.036655	1275.335880	19.073997
46.658105	1269.177494	19.079015
46.735506	1266.832914	19.084032
46.887916	1256.845343	19.089050
46.628106	1269.385468	19.094067
46.663776	1286.684866	19.099085
46.902661	1296.866098	19.104103
47.124743	1299.937235	19.109120
47.459312	1290.950172	19.114138
47.328749	1300.841799	19.119155
47.485687	1297.245481	19.124173
47.079203	1297.010122	19.129191
47.321750	1293.660649	19.134208
47.610912	1288.334986	19.139226
47.633960	1300.810190	19.144243
47.336422	1295.474587	19.149261
47.394860	1296.157504	19.154279
47.379075	1291.953577	19.159296
47.806094	1291.529417	19.164314
47.397062	1301.538807	19.169331
47.688191	1296.586038	19.174349
47.367985	1295.900178	19.179367
47.379537	1296.257400	19.184384
47.664691	1295.088239	19.189402
47.473766	1301.761566	19.194419
47.592218	1308.902559	19.199437
47.972539	1321.119412	19.204455
48.026116	1325.336157	19.209472
48.200705	1320.222365	19.214490
48.058001	1324.878297	19.219507
48.442635	1320.823805	19.224525
47.953580	1323.875299	19.229543
47.746857	1325.428490	19.234560
48.108349	1317.001514	19.239578
48.228075	1321.253761	19.244595
48.069641	1324.837510	19.249613
48.241923	1319.867405	19.254631
48.420825	1329.135375	19.259648
48.331807	1322.696353	19.264666
48.630884	1349.128062	19.269683
48.770634	1342.200763	19.274701
48.728613	1335.440177	19.279719
48.415849	1331.620055	19.284736
48.660547	1339.384243	19.289754
48.297907	1348.548590	19.294771
48.430544	1354.632937	19.299789
48.599218	1343.156416	19.304807
48.761788	1342.525259	19.309824
48.897305	1348.237084	19.314842
48.629196	1351.794906	19.319859
48.932330	1352.283767	19.324877
48.983094	1371.618530	19.329895
49.247597	1368.535088	19.334912
49.612736	1361.611798	19.339930
49.770028	1367.062941	19.344947
49.706430	1342.543142	19.349965
49.740578	1335.965611	19.354983
49.415346	1334.907752	19.360000
49.685942	1327.702104	19.365018
49.675457	1334.146752	19.370035
49.675792	1330.106284	19.375053
49.771820	1327.320428	19.380071
49.394172	1326.651559	19.385088
49.508578	1328.269685	19.390106
49.569630	1332.176931	19.395123
49.572719	1347.910946	19.400141
50.022258	1350.572782	19.405159
49.618040	1358.548759	19.410176
50.098151	1355.123323	19.415194
50.089169	1358.015018	19.420211
50.002763	1349.372428	19.425229
50.117948	1357.315155	19.430247
49.982690	1364.735976	19.435264
50.373883	1355.380450	19.440282
50.254033	1357.496418	19.445299
50.238023	1351.079152	19.450317
50.427705	1358.704824	19.455335
49.933885	1357.951647	19.460352
50.430665	1352.261667	19.465370
50.332496	1360.166496	19.470387
50.298866	1367.513011	19.475405
50.598591	1380.994817	19.480423
50.363754	1390.175034	19.485440
50.814034	1381.977807	19.490458
50.774082	1383.578192	19.495475
50.679746	1384.396252	19.500493
51.100138	1385.403488	19.505511
50.833214	1398.016548	19.510528
50.903695	1377.100838	19.515546
50.844430	1389.920449	19.520563
50.905302	1376.061383	19.525581
51.094389	1381.714351	19.530599
51.069518	1389.202337	19.535616
50.807323	1387.624987	19.540634
51.193308	1389.036342	19.545651
51.019049	1397.912441	19.550669
51.328829	1407.178866	19.555687
51.204594	1410.190047	19.560704
51.539373	1403.610740	19.565722
51.627096	1405.905334	19.570739
51.970703	1406.548518	19.575757
52.032808	1399.122637	19.580775
51.775381	1400.058646	19.585792
52.390776	1390.438812	19.590810
51.917314	1378.151670	19.595827
51.725184	1371.474979	19.600845
51.874751	1370.592433	19.605863
51.936282	1375.851958	19.610880
52.361345	1376.331655	19.615898
52.015996	1364.715429	19.620915
51.807894	1353.181603	19.625933
52.131907	1366.908586	19.630951
52.085542	1387.324794	19.635968
52.535644	1388.185775	19.640986
52.008909	1390.674629	19.646003
52.412850	1392.344426	19.651021
52.498465	1388.254390	19.656039
52.210194	1387.226233	19.661056
52.418981	1384.268942	19.666074
52.202298	1388.132426	19.671091
52.344367	1383.123604	19.676109
52.395941	1381.595086	19.681127
52.495237	1392.060515	19.686144
52.519073	1390.410606	19.691162
52.682288	1399.664287	19.696179
52.917862	1416.471678	19.701197
53.144122	1410.191437	19.706215
53.053756	1418.883973	19.711232
53.158439	1412.564807	19.716250
52.985320	1395.444101	19.721267
52.842018	1403.554455	19.726285
53.245433	1410.973898	19.731303
52.793094	1414.255549	19.736320
53.136889	1412.541635	19.741338
53.044493	1409.938930	19.746355
53.022173	1415.476523	19.751373
53.527280	1411.553634	19.756391
53.531958	1412.267899	19.761408
53.549134	1407.935255	19.766426
53.520350	1411.292833	19.771443
53.097527	1414.715658	19.776461
54.000960	1416.046455	19.781479
53.701330	1429.352745	19.786496
53.802498	1423.251871	19.791514
53.745700	1438.879361	19.796531
53.981841	1425.293196	19.801549
53.648697	1419.766202	19.806567
53.587541	1438.323918	19.811584
53.905618	1429.117461	19.816602
53.953331	1427.693121	19.821619
54.014378	1428.097268	19.826637
54.135646	1420.760792	19.831655
54.454911	1441.846840	19.836672
54.599112	1446.224596	19.841690
54.487057	1438.282262	19.846707
54.647041	1431.998025	19.851725
54.655748	1425.011285	19.856743
54.400287	1422.003299	19.861760
54.498264	1433.670934	19.866778
54.630860	1446.691499	19.871795
54.414882	1453.152505	19.876813
54.863628	1450.489325	19.881831
54.603821	1456.621765	19.886848
54.983272	1443.198862	19.891866
55.033924	1452.807038	19.896883
55.009866	1449.961910	19.901901
55.056605	1447.458995	19.906919
54.619740	1451.077459	19.911936
55.061151	1456.175292	19.916954
55.259984	1446.431486	19.921971
55.109889	1455.252830	19.926989
55.144286	1447.978757	19.932007
55.068453	1453.329950	19.937024
55.120668	1472.705544	19.942042
55.604349	1467.725563	19.947059
55.236802	1472.648296	19.952077
55.351831	1474.764364	19.957095
55.157172	1482.134053	19.962112
55.661422	1481.593165	19.967130
55.636801	1469.701314	19.972147
55.552376	1476.094484	19.977165
55.812996	1471.725450	19.982183
56.039083	1475.292414	19.987200
55.919655	1465.428460	19.992218
56.060413	1473.586697	19.997235
56.141613	1489.440993	20.002253
56.040268	1498.001140	20.007271
56.128169	1498.113442	20.012288
56.316122	1496.393827	20.017306
56.504718	1494.019778	20.022323
56.441345	1504.280329	20.027341
56.607871	1492.876099	20.032359
56.575044	1495.013109	20.037376
56.886130	1490.979020	20.042394
56.877196	1476.395204	20.047411
56.711613	1461.579467	20.052429
56.924013	1450.122792	20.057447
56.901323	1459.253749	20.062464
56.743960	1458.488162	20.067482
56.758979	1452.954294	20.072499
56.743934	1458.964711	20.077517
57.039822	1464.067352	20.082535
57.258213	1480.734746	20.087552
57.152088	1485.200024	20.092570
57.177729	1473.312839	20.097587
57.109227	1489.747039	20.102605
57.304303	1485.539641	20.107623
56.619179	1499.673598	20.112640
57.375906	1487.014957	20.117658
56.991388	1487.788157	20.122675
56.879456	1490.354799	20.127693
57.073977	1493.215580	20.132711
57.449629	1499.605414	20.137728
57.456021	1511.773311	20.142746
57.543180	1505.827087	20.147763
57.259672	1515.131971	20.152781
57.632551	1512.791972	20.157799
57.570761	1516.662124	20.162816
57.925576	1524.131402	20.167834
57.879471	1535.370216	20.172851
57.900143	1532.607036	20.177869
58.254256	1531.081559	20.182887
58.458678	1530.756457	20.187904
58.573219	1535.054110	20.192922
58.672314	1530.501174	20.197939
58.497711	1534.140011	20.202957
58.580554	1523.716544	20.207975
58.514489	1527.038588	20.212992
58.709997	1509.564987	20.218010
58.677612	1503.049582	20.223027
58.594166	1503.007579	20.228045
58.485437	1509.342583	20.233063
58.741679	1524.704547	20.238080
58.690678	1521.806780	20.243098
58.744393	1514.642863	20.248115
58.996110	1526.962277	20.253133
59.024493	1516.188384	20.258151
58.989970	1518.819378	20.263168
58.853613	1519.433772	20.268186
59.027233	1518.679520	20.273203
58.829028	1525.986431	20.278221
58.975871	1522.214961	20.283239
58.581336	1529.059501	20.288256
58.786722	1552.981091	20.293274
59.065456	1550.391320	20.298291
59.194286	1552.837398	20.303309
59.094997	1546.783841	20.308327
59.333766	1559.243613	20.313344
59.489502	1570.258480	20.318362
60.224282	1567.082958	20.323379
59.744464	1580.197164	20.328397
60.418672	1564.696212	20.333415
60.439070	1573.686244	20.338432
60.457094	1553.381345	20.343450
60.164730	1543.206606	20.348467
60.336926	1543.014399	20.353485
60.051523	1531.555050	20.358503
60.053893	1540.237024	20.363520
59.858621	1533.837160	20.368538
60.380418	1530.681162	20.373555
60.206687	1548.324186	20.378573
60.420420	1559.442040	20.383591
60.641149	1556.288645	20.388608
60.243528	1563.172292	20.393626
60.761984	1553.584946	20.398643
60.574241	1564.516130	20.403661
60.621522	1562.470982	20.408679
60.379037	1567.890360	20.413696
60.739440	1560.673278	20.418714
60.815715	1549.825684	20.423731
60.426889	1561.265358	20.428749
60.900051	1563.783164	20.433767
60.962644	1574.624086	20.438784
60.963427	1578.844524	20.443802
61.167062	1583.549486	20.448819
61.166115	1587.997379	20.453837
61.190109	1581.957253	20.458855
61.342571	1579.256102	20.463872
61.063666	1586.526797	20.468890
61.527465	1588.385526	20.473907
61.283709	1608.981167	20.478925
61.756074	1614.786923	20.483943
61.786874	1608.014948	20.488960
62.009398	1611.884898	20.493978
62.050786	1619.088402	20.498995
62.157989	1618.540025	20.504013
62.140957	1613.988970	20.509031
62.592212	1620.806891	20.514048
62.186027	1601.221780	20.519066
62.199545	1587.105404	20.524083
61.925772	1591.070911	20.529101
61.983596	1597.959083	20.534119
62.394673	1600.987571	20.539136
62.221048	1606.812492	20.544154
62.341437	1609.436355	20.549171
62.764335	1604.934114	20.554189
62.485740	1607.741364	20.559207
62.472137	1603.422029	20.564224
62.255048	1610.435255	20.569242
62.614696	1610.277364	20.574259
62.499239	1614.346979	20.579277
62.504430	1629.612820	20.584295
62.632335	1633.303166	20.589312
62.526183	1632.057040	20.594330
62.806796	1628.385838	20.599347
62.932075	1634.300253	20.604365
63.167994	1647.893253	20.609383
63.378203	1656.213317	20.614400
63.528557	1658.464901	20.619418
63.738134	1652.574336	20.624435
63.542298	1638.401239	20.629453
63.663177	1625.117451	20.634471
63.872904	1624.908005	20.639488
63.610822	1618.180190	20.644506
63.736666	1618.608653	20.649523
63.597246	1628.009038	20.654541
63.629581	1631.685680	20.659559
64.052679	1634.389742	20.664576
64.016332	1651.439265	20.669594
64.000089	1651.119202	20.674611
63.976597	1651.086169	20.679629
64.128998	1652.950797	20.684647
64.293675	1649.468472	20.689664
64.167224	1650.076113	20.694682
64.323848	1649.854200	20.699699
64.421890	1649.776633	20.704717
64.336591	1645.832547	20.709735
64.283826	1644.807109	20.714752
64.219902	1646.157945	20.719770
64.541567	1637.772431	20.724787
64.349822	1647.415352	20.729805
64.341277	1657.307868	20.734823
64.858783	1664.506574	20.739840
64.502879	1669.320746	20.744858
64.916673	1669.199953	20.749875
64.774932	1684.670494	20.754893
64.609449	1672.886062	20.759911
64.717458	1676.388373	20.764928
65.036670	1702.216560	20.769946
65.273354	1698.209698	20.774963
65.127211	1706.139182	20.779981
65.352602	1705.829896	20.784999
65.522646	1709.227060	20.790016
65.317201	1706.734363	20.795034
65.625801	1694.675352	20.800051
65.879402	1695.694087	20.805069
65.758567	1693.060610	20.810087
65.881639	1699.448255	20.815104
65.523676	1694.766224	20.820122
65.745221	1705.872654	20.825139
65.765271	1724.491677	20.830157
66.216566	1718.171689	20.835175
66.012210	1723.448585	20.840192
66.167793	1728.478481	20.845210
66.404321	1724.071239	20.850227
66.352592	1720.835757	20.855245
66.220065	1723.781442	20.860263
66.375524	1717.822646	20.865280
66.367022	1723.337982	20.870298
66.530289	1706.827777	20.875315
66.766208	1712.604611	20.880333
66.817383	1716.158073	20.885351
66.752267	1707.977117	20.890368
66.647996	1729.743536	20.895386
67.002811	1734.686508	20.900403
67.265667	1734.459210	20.905421
67.338847	1728.622696	20.910439
67.740473	1735.770937	20.915456
67.379745	1719.464411	20.920474
67.174668	1704.756163	20.925491
67.264738	1705.901582	20.930509
67.394864	1720.923990	20.935527
67.800181	1715.454146	20.940544
67.872405	1728.152657	20.945562
67.985014	1723.889164	20.950579
67.296105	1706.651152	20.955597
67.480140	1706.416432	20.960615
67.836281	1718.772647	20.965632
67.562217	1733.542303	20.970650
67.743026	1738.195580	20.975667
67.823112	1734.191015	20.980685
67.387135	1742.162996	20.985703
67.600164	1735.998989	20.990720
67.626223	1736.892014	20.995738
68.027239	1743.847444	21.000755
68.100295	1745.544904	21.005773
67.898419	1753.289149	21.010791
67.903843	1750.478061	21.015808
68.252580	1768.306876	21.020826
68.409249	1776.644138	21.025843
68.369995	1776.699542	21.030861
68.902190	1778.266650	21.035879
69.123134	1775.602553	21.040896
68.880819	1778.669971	21.045914
68.591091	1778.052271	21.050931
68.814910	1773.106166	21.055949
69.047962	1777.164182	21.060967
69.184618	1770.798631	21.065984
68.935196	1772.818784	21.071002
69.409254	1774.494733	21.076019
69.214038	1773.101923	21.081037
69.154791	1789.719950	21.086055
69.526247	1795.642092	21.091072
69.526107	1804.615579	21.096090
69.566957	1793.635882	21.101107
69.796811	1799.668088	21.106125
69.514161	1801.894143	21.111143
70.227831	1794.841300	21.116160
69.892369	1793.257139	21.121178
69.995738	1796.449610	21.126195
70.079839	1792.430979	21.131213
69.990915	1790.940646	21.136231
69.926288	1786.008832	21.141248
70.028684	1791.474728	21.146266
70.315243	1801.645644	21.151283
70.459495	1814.429152	21.156301
70.447213	1821.840459	21.161319
70.561601	1815.043923	21.166336
70.609387	1823.416167	21.171354
70.550418	1819.491299	21.176371
70.604581	1819.637143	21.181389
70.640381	1819.662797	21.186407
70.738987	1816.021293	21.191424
70.714912	1818.308083	21.196442
70.686483	1815.534085	21.201459
70.862940	1822.475157	21.206477
71.162735	1838.142825	21.211495
71.247770	1831.910996	21.216512
71.496661	1835.767975	21.221530
71.466562	1837.599851	21.226547
71.748141	1830.731136	21.231565
71.309959	1830.850231	21.236583
71.736191	1828.195836	21.241600
71.581471	1833.943693	21.246618
71.418312	1839.066166	21.251635
71.671065	1834.516047	21.256653
71.496467	1830.942612	21.261671
71.694280	1847.840978	21.266688
71.995227	1860.328495	21.271706
71.839147	1861.907998	21.276723
71.979238	1865.669612	21.281741
71.672731	1867.632692	21.286759
72.078747	1857.925586	21.291776
71.944779	1860.013250	21.296794
72.452822	1862.903686	21.301811
73.200465	1870.181315	21.306829
72.623030	1868.755324	21.311847
72.987893	1852.904513	21.316864
73.024008	1846.225650	21.321882
72.925457	1849.419675	21.326899
73.099909	1839.442648	21.331917
73.026873	1838.627645	21.336935
73.053620	1843.429300	21.341952
73.055146	1843.331492	21.346970
73.108232	1851.019003	21.351987
73.361250	1835.691855	21.357005
72.907151	1850.182371	21.362023
73.146082	1856.199316	21.367040
73.373127	1869.687285	21.372058
73.403753	1878.033660	21.377075
73.732670	1873.535487	21.382093
73.396971	1875.492772	21.387111
73.663091	1869.057318	21.392128
73.586249	1868.898075	21.397146
73.407585	1864.776081	21.402163
73.847445	1879.324908	21.407181
73.851031	1892.392407	21.412199
74.076246	1894.442650	21.417216
74.100642	1896.898595	21.422234
73.974160	1894.348303	21.427251
74.455917	1893.323324	21.432269
74.417181	1899.139798	21.437287
74.209358	1890.972138	21.442304
74.548100	1894.105184	21.447322
74.223801	1898.587807	21.452339
74.866636	1907.392685	21.457357
74.547190	1922.884225	21.462375
74.891826	1922.037857	21.467392
75.084571	1916.921258	21.472410
75.264824	1924.025924	21.477427
75.382158	1916.602856	21.482445
75.221399	1920.638319	21.487463
75.491538	1909.236314	21.492480
75.332694	1917.074698	21.497498
75.623576	1922.466911	21.502515
75.488593	1909.322491	21.507533
75.561019	1922.199085	21.512551
75.905004	1916.114115	21.517568
75.705439	1909.964023	21.522586
75.593278	1920.204186	21.527603
75.818320	1913.578661	21.532621
75.728906	1914.422704	21.537639
75.653995	1915.010797	21.542656
75.712282	1909.069593	21.547674
76.072158	1909.885702	21.552691
76.200181	1921.557786	21.557709
76.228182	1935.796899	21.562727
76.206321	1950.695478	21.567744
76.167971	1944.270248	21.572762
76.290288	1937.123125	21.577779
76.626560	1934.741488	21.582797
76.405261	1938.526735	21.587815
76.584643	1934.657651	21.592832
76.537392	1935.810471	21.597850
76.693354	1961.517299	21.602867
76.965982	1954.171653	21.607885
76.597137	1964.345288	21.612903
76.748819	1956.618474	21.617920
76.688070	1958.420792	21.622938
76.983478	1961.111409	21.627955
77.334185	1975.663277	21.632973
77.547122	1980.835338	21.637991
77.612149	1978.097020	21.643008
77.759007	1975.924697	21.648026
77.831403	1984.216180	21.653043
77.775471	1981.115988	21.658061
77.566998	1989.417364	21.663079
77.954097	1981.407851	21.668096
78.049302	1984.841877	21.673114
78.048210	1982.642474	21.678131
78.048088	1970.032382	21.683149
77.820710	1987.016657	21.688167
78.186368	1981.632817	21.693184
78.068052	1981.716274	21.698202
78.220030	1982.644765	21.703219
78.063004	1981.816495	21.708237
78.163436	2000.965075	21.713255
78.035672	2009.454678	21.718272
78.612554	2010.904962	21.723290
78.449165	2008.541083	21.728307
78.501102	2007.751048	21.733325
78.661021	2032.896693	21.738343
79.126570	2029.780228	21.743360
79.229214	2036.316676	21.748378
79.004909	2047.205432	21.753395
79.544470	2031.913721	21.758413
79.352795	2025.778026	21.763431
79.791550	2031.644627	21.768448
79.891732	2025.782271	21.773466
79.690519	2022.920306	21.778483
80.002049	2032.967552	21.783501
79.845627	2039.207514	21.788519
79.898211	2022.588525	21.793536
79.894053	2015.133950	21.798554
79.653673	2027.383664	21.803571
80.250818	2018.580669	21.808589
79.974949	2024.239203	21.813607
79.767644	2018.471858	21.818624
80.222196	2027.232388	21.823642
80.309874	2044.946081	21.828659
80.455629	2051.953759	21.833677
79.991175	2049.529089	21.838695
80.436187	2059.492438	21.843712
80.666523	2047.568952	21.848730
80.575189	2053.076466	21.853747
80.691123	2044.267304	21.858765
80.755644	2054.432236	21.863783
80.899555	2074.932809	21.868800
80.583348	2074.162780	21.873818
80.893070	2080.564562	21.878835
81.184156	2078.954585	21.883853
81.459353	2080.022529	21.888871
81.302274	2071.606599	21.893888
81.594878	2071.850766	21.898906
81.883657	2089.068598	21.903923
82.089748	2084.820237	21.908941
81.970514	2080.063126	21.913959
81.600913	2075.237230	21.918976
82.237816	2078.382760	21.923994
82.193791	2094.445818	21.929011
82.378589	2086.372106	21.934029
82.112797	2069.732157	21.939047
82.280978	2084.440338	21.944064
82.400128	2083.214747	21.949082
82.053700	2092.459917	21.954099
82.289226	2080.182386	21.959117
82.376030	2077.505801	21.964135
82.074388	2080.852008	21.969152
82.608042	2086.979699	21.974170
82.677874	2104.909809	21.979187
82.860341	2112.823280	21.984205
82.714818	2118.354750	21.989223
82.598029	2123.942885	21.994240
82.846327	2114.830653	21.999258
82.961983	2115.547049	22.004275
83.115364	2106.372977	22.009293
83.239997	2121.273055	22.014311
83.513454	2133.765739	22.019328
83.590220	2134.162972	22.024346
83.766791	2133.287332	22.029363
83.866706	2128.152569	22.034381
84.123070	2136.843217	22.039399
83.856901	2137.855520	22.044416
84.329387	2139.900290	22.049434
83.914904	2132.967159	22.054451
84.081856	2137.723248	22.059469
83.994903	2130.042554	22.064487
84.022352	2139.850675	22.069504
84.310683	2127.573419	22.074522
84.056396	2128.467608	22.079539
84.290796	2137.541435	22.084557
84.279367	2147.651678	22.089575
84.337052	2165.782696	22.094592
84.780557	2153.454135	22.099610
84.177428	2166.147498	22.104627
84.730873	2158.267840	22.109645
84.914029	2182.227155	22.114663
84.766192	2183.277351	22.119680
85.278946	2191.702340	22.124698
85.159293	2195.879892	22.129715
85.154173	2188.925021	22.134733
85.094503	2192.122914	22.139751
85.452836	2194.188561	22.144768
85.837834	2205.038356	22.149786
86.101527	2206.940533	22.154803
85.939957	2207.877251	22.159821
86.062994	2213.382794	22.164839
86.097813	2213.462157	22.169856
86.181472	2197.509124	22.174874
86.067131	2213.278816	22.179891
86.248391	2204.503237	22.184909
86.483640	2207.984601	22.189927
86.140752	2204.826754	22.194944
86.473410	2200.446378	22.199962
86.659840	2202.203860	22.204979
86.610373	2202.716488	22.209997
86.634702	2207.193445	22.215015
86.374686	2197.759800	22.220032
86.841705	2215.603406	22.225050
86.677863	2222.537220	22.230067
87.196665	2233.943647	22.235085
87.333994	2230.730694	22.240103
87.013912	2238.846735	22.245120
87.166155	2221.021216	22.250138
87.253143	2236.754053	22.255155
87.428066	2246.364981	22.260173
87.807412	2255.085729	22.265191
87.933604	2252.139982	22.270208
87.994019	2255.756609	22.275226
87.800335	2256.004520	22.280243
88.132205	2257.773363	22.285261
88.136449	2251.800029	22.290279
87.995112	2253.057431	22.295296
88.200235	2244.379458	22.300314
88.289615	2242.435522	22.305331
88.312511	2249.403393	22.310349
88.450110	2239.394022	22.315367
88.297764	2250.624958	22.320384
88.431109	2258.400961	22.325402
88.378816	2273.095430	22.330419
88.377329	2276.605376	22.335437
88.460160	2271.489536	22.340455
88.426193	2277.261660	22.345472
89.067323	2290.968457	22.350490
89.000824	2299.721316	22.355507
89.214734	2309.509301	22.360525
89.391553	2299.483161	22.365543
89.331656	2304.460336	22.370560
89.783371	2294.723740	22.375578
89.432088	2294.214243	22.380595
89.652186	2302.932251	22.385613
89.871935	2283.115859	22.390631
89.754909	2290.493941	22.395648
90.016297	2292.384306	22.400666
90.048557	2314.388005	22.405683
90.025814	2318.483398	22.410701
90.432419	2313.539145	22.415719
90.122258	2323.861965	22.420736
90.474246	2317.513691	22.425754
90.448324	2313.331245	22.430771
90.336429	2315.649183	22.435789
90.637096	2307.531763	22.440807
90.334786	2324.163832	22.445824
91.309388	2330.707220	22.450842
90.970809	2340.967824	22.455859
90.901399	2342.791306	22.460877
91.343771	2344.660767	22.465895
91.125968	2348.069923	22.470912
91.469275	2336.512573	22.475930
91.665886	2346.486526	22.480947
91.351897	2343.442375	22.485965
91.705875	2334.880264	22.490983
91.478591	2341.475011	22.496000
91.611968	2338.186702	22.501018
91.539069	2352.961040	22.506035
91.867209	2362.787629	22.511053
91.710611	2356.662924	22.516071
92.007434	2372.897405	22.521088
92.203525	2362.581010	22.526106
91.962602	2370.037521	22.531123
92.155390	2386.443187	22.536141
92.509147	2401.055978	22.541159
92.500225	2394.750499	22.546176
92.683845	2395.664328	22.551194
92.844474	2398.834844	22.556211
92.669618	2400.408847	22.561229
93.117851	2383.823576	22.566247
92.855232	2395.726059	22.571264
92.964114	2407.036303	22.576282
92.976365	2414.003254	22.581299
93.057021	2412.506437	22.586317
93.587508	2406.079357	22.591335
93.411141	2416.009592	22.596352
93.512509	2408.841311	22.601370
93.678817	2427.204662	22.606387
93.822721	2436.075919	22.611405
94.313659	2433.360315	22.616423
93.863027	2447.624417	22.621440
94.335488	2441.604985	22.626458
94.138952	2442.329777	22.631475
94.056554	2438.279490	22.636493
94.551877	2432.913400	22.641511
94.358310	2448.622821	22.646528
94.514640	2440.103615	22.651546
94.752095	2434.990469	22.656563
94.860967	2446.156640	22.661581
95.247784	2452.846618	22.666599
94.881886	2447.476258	22.671616
94.675745	2442.790514	22.676634
95.145302	2449.478209	22.681651
95.151886	2448.105470	22.686669
95.423295	2449.516608	22.691687
95.275911	2443.479719	22.696704
95.358177	2443.216955	22.701722
95.474093	2450.579775	22.706739
95.331561	2450.284543	22.711757
95.576643	2443.517672	22.716775
95.454037	2469.723853	22.721792
95.697576	2472.322356	22.726810
95.684552	2472.071039	22.731827
95.643361	2478.246819	22.736845
95.961307	2477.500518	22.741863
95.988935	2497.102342	22.746880
96.240373	2504.501019	22.751898
96.455239	2500.399923	22.756915
96.174149	2502.751021	22.761933
96.630282	2513.655402	22.766951
96.846977	2527.543715	22.771968
96.898283	2526.280894	22.776986
97.154186	2526.598081	22.782003
96.993158	2531.329457	22.787021
97.704123	2524.394465	22.792039
97.298844	2525.344779	22.797056
97.765185	2529.410828	22.802074
97.890826	2530.983913	22.807091
97.290533	2532.603564	22.812109
97.763707	2519.289820	22.817127
97.160084	2525.636305	22.822144
97.625621	2535.709958	22.827162
97.983638	2537.177635	22.832179
97.976463	2550.262823	22.837197
98.164745	2546.357861	22.842215
98.187174	2545.890817	22.847232
98.202308	2543.380360	22.852250
98.200494	2559.203428	22.857267
98.349651	2578.008409	22.862285
98.813062	2571.984520	22.867303
98.478896	2578.571470	22.872320
98.916848	2575.190555	22.877338
99.244269	2569.519127	22.882355
98.946555	2574.853107	22.887373
99.431278	2567.844130	22.892391
99.596938	2591.349463	22.897408
99.534403	2586.265070	22.902426
99.613418	2585.022462	22.907443
99.455938	2603.537669	22.912461
99.849034	2590.668256	22.917479
99.694219	2598.598446	22.922496
99.779652	2597.853628	22.927514
100.186870	2592.973758	22.932531
99.925442	2596.666982	22.937549
99.900090	2593.694684	22.942567
100.224814	2596.265198	22.947584
100.381616	2616.904125	22.952602
100.570080	2618.316807	22.957619
100.511525	2629.239552	22.962637
100.702843	2615.788522	22.967655
100.784157	2628.950470	22.972672
100.698555	2616.492994	22.977690
100.741754	2615.539404	22.982707
101.076445	2628.243230	22.987725
101.421163	2627.672818	22.992743
101.327611	2633.649834	22.997760
101.252022	2647.064564	23.002778
101.408633	2644.358213	23.007795
101.305251	2649.098192	23.012813
101.474227	2640.274005	23.017831
101.656351	2646.982997	23.022848
101.538523	2640.072965	23.027866
101.866892	2639.360368	23.032883
101.497607	2661.619243	23.037901
102.416854	2661.259240	23.042919
102.089215	2663.694452	23.047936
102.185706	2673.506046	23.052954
102.485142	2666.805676	23.057971
102.385472	2664.483905	23.062989
102.292119	2663.289517	23.068007
102.476592	2683.370367	23.073024
102.258930	2691.654342	23.078042
102.602187	2683.079643	23.083059
102.828844	2696.260107	23.088077
102.691923	2723.708153	23.093095
103.079137	2722.477109	23.098112
103.094788	2722.058035	23.103130
103.424318	2721.349180	23.108147
103.408220	2725.755414	23.113165
103.656538	2726.399477	23.118183
103.985496	2742.849514	23.123200
104.114430	2747.903841	23.128218
104.593894	2740.899596	23.133235
104.147992	2738.693805	23.138253
104.292324	2734.313359	23.143271
104.382104	2735.928232	23.148288
104.534579	2736.936616	23.153306
104.595126	2725.350199	23.158323
104.489645	2738.698691	23.163341
104.896883	2731.889100	23.168359
104.951852	2733.384923	23.173376
104.811252	2733.026762	23.178394
105.061318	2747.954315	23.183411
105.056540	2757.248436	23.188429
105.046995	2763.543508	23.193447
105.198199	2760.410440	23.198464
105.109693	2766.723706	23.203482
105.084398	2765.900748	23.208499
105.202663	2777.220339	23.213517
105.780423	2789.617495	23.218535
105.702019	2798.351737	23.223552
105.805148	2801.782270	23.228570
105.920730	2803.113721	23.233587
106.047525	2817.321534	23.238605
106.168212	2821.778383	23.243623
106.660154	2828.137707	23.248640
106.271237	2825.346042	23.253658
106.460674	2824.176480	23.258675
106.404529	2827.133348	23.263693
106.964935	2832.612369	23.268711
107.044915	2838.058328	23.273728
106.753673	2838.357048	23.278746
107.230365	2836.999360	23.283763
107.119935	2837.560688	23.288781
107.274839	2839.045488	23.293799
107.465842	2856.107511	23.298816
107.656634	2858.637641	23.303834
107.612051	2857.969853	23.308851
107.524209	2872.857796	23.313869
107.935951	2862.747908	23.318887
108.244752	2854.651302	23.323904
107.880985	2867.091406	23.328922
108.372620	2878.872919	23.333939
108.211028	2887.157557	23.338957
108.357897	2880.216193	23.343975
108.493678	2889.596184	23.348992
108.520948	2882.113942	23.354010
108.642694	2884.330283	23.359027
108.600859	2883.652590	23.364045
108.664118	2896.705933	23.369063
109.106963	2894.895537	23.374080
109.417949	2908.405162	23.379098
109.808922	2905.334738	23.384115
109.357035	2915.211686	23.389133
109.191779	2912.116415	23.394151
109.463164	2913.918187	23.399168
109.416585	2922.503909	23.404186
109.644566	2912.610257	23.409203
109.472738	2925.700578	23.414221
109.769315	2932.456498	23.419239
109.960498	2940.785522	23.424256
109.683715	2944.083694	23.429274
110.037786	2956.519202	23.434291
110.118640	2966.232378	23.439309
110.211398	2973.882377	23.444327
110.439292	2977.537984	23.449344
110.585975	2992.761655	23.454362
110.894071	2999.155426	23.459379
111.095264	3002.860346	23.464397
110.773516	2999.540157	23.469415
111.522662	2991.541456	23.474432
111.491274	2997.073238	23.479450
111.721545	2987.226802	23.484467
111.358940	2998.693893	23.489485
111.444954	3009.694159	23.494503
112.179815	3016.157449	23.499520
112.156092	3017.261566	23.504538
112.204833	3014.303696	23.509555
112.119942	3018.168594	23.514573
112.168718	3022.343679	23.519591
112.736739	3011.363252	23.524608
112.265269	3025.823472	23.529626
112.509692	3026.639863	23.534643
112.477920	3041.856510	23.539661
112.450488	3045.227604	23.544679
112.654307	3046.233807	23.549696
112.690817	3050.468416	23.554714
113.042153	3060.510133	23.559731
113.309960	3064.707237	23.564749
113.001744	3073.139884	23.569767
113.555004	3067.437580	23.574784
113.546082	3091.635235	23.579802
113.673359	3092.664746	23.584819
113.767263	3097.462362	23.589837
113.732843	3106.149725	23.594855
113.814461	3102.410332	23.599872
113.804858	3116.141343	23.604890
114.075358	3119.294998	23.609907
114.070867	3129.751220	23.614925
114.227044	3126.123112	23.619943
114.599034	3128.034643	23.624960
114.674208	3141.087793	23.629978
115.116697	3144.151947	23.634995
115.232089	3144.662509	23.640013
115.378136	3154.307917	23.645031
115.810577	3142.892713	23.650048
115.982084	3141.594586	23.655066
115.980781	3139.873844	23.660083
115.745035	3139.916110	23.665101
115.820243	3137.266071	23.670119
115.968522	3138.739004	23.675136
116.020376	3146.237969	23.680154
115.884545	3138.959004	23.685171
116.172026	3140.985327	23.690189
116.200315	3146.336397	23.695207
116.277433	3132.327789	23.700224
116.356828	3135.791462	23.705242
116.343644	3151.594176	23.710259
116.405527	3167.216743	23.715277
116.202615	3175.327647	23.720295
116.614665	3174.205463	23.725312
116.439443	3193.707874	23.730330
116.616242	3184.710808	23.735347
116.888745	3204.802167	23.740365
117.095194	3214.130491	23.745383
117.200400	3221.133205	23.750400
117.008559	3233.071854	23.755418
117.266254	3232.635530	23.760435
117.525885	3241.564866	23.765453
117.848268	3251.248074	23.770471
118.309319	3246.165764	23.775488
117.956653	3246.225420	23.780506
117.853598	3258.759691	23.785523
118.623052	3267.476272	23.790541
118.418451	3272.391089	23.795559
119.021378	3263.178134	23.800576
119.008412	3270.663873	23.805594
119.564325	3256.820396	23.810611
119.590194	3254.179293	23.815629
119.666025	3256.177675	23.820647
119.802952	3258.724664	23.825664
119.599314	3259.622339	23.830682
119.826563	3255.969440	23.835699
119.996638	3249.819040	23.840717
119.442698	3255.198821	23.845735
119.860307	3252.853923	23.850752
120.060673	3257.029565	23.855770
120.084924	3257.000829	23.860787
120.027989	3270.251963	23.865805
120.207454	3279.742293	23.870823
120.216899	3283.459340	23.875840
120.225765	3290.129571	23.880858
120.270805	3303.643015	23.885875
120.176811	3310.113725	23.890893
120.591049	3320.385774	23.895911
120.741891	3325.809540	23.900928
120.610152	3339.635781	23.905946
121.153821	3346.586825	23.910963
121.188050	3349.648528	23.915981
121.651089	3364.727654	23.920999
121.747644	3370.626620	23.926016
121.588399	3380.766466	23.931034
121.750718	3372.155201	23.936051
121.869873	3371.123628	23.941069
122.195032	3395.141622	23.946087
122.241578	3399.505388	23.951104
122.450666	3403.569376	23.956122
122.440785	3398.712643	23.961139
122.712967	3396.144922	23.966157
122.817142	3404.395282	23.971175
122.971938	3416.926757	23.976192
122.938771	3424.033584	23.981210
123.123676	3425.286675	23.986227
123.360638	3419.701582	23.991245
123.597072	3432.166397	23.996263
123.788648	3418.363019	24.001280
123.616671	3421.914443	24.006298
123.613471	3429.937288	24.011315
123.764194	3431.072008	24.016333
123.936643	3443.052877	24.021351
124.316059	3441.410818	24.026368
124.364215	3450.206369	24.031386
124.197220	3452.917896	24.036403
124.101356	3442.892466	24.041421
124.564197	3468.825810	24.046439
124.263495	3463.445089	24.051456
124.493100	3474.600670	24.056474
124.648050	3476.519043	24.061491
124.888401	3475.066167	24.066509
125.114864	3495.774654	24.071527
125.320533	3494.641731	24.076544
125.447957	3498.336146	24.081562
125.883979	3504.054140	24.086579
125.805068	3492.299669	24.091597
125.728611	3499.986998	24.096615
126.187988	3504.182037	24.101632
125.964273	3524.946195	24.106650
125.951440	3527.757424	24.111667
126.535566	3526.625234	24.116685
126.467337	3529.992949	24.121703
126.320169	3519.112862	24.126720
126.446395	3531.810203	24.131738
126.639204	3546.970472	24.136755
126.899565	3543.635295	24.141773
127.157554	3559.867601	24.146791
127.448156	3539.145254	24.151808
127.067270	3557.973810	24.156826
127.307912	3573.816038	24.161843
127.663141	3574.651521	24.166861
127.582130	3579.813723	24.171879
127.682155	3573.910651	24.176896
128.017036	3587.529523	24.181914
127.871614	3601.314159	24.186931
128.412305	3600.994379	24.191949
128.628856	3602.066238	24.196967
128.438234	3605.110487	24.201984
128.613272	3606.947587	24.207002
128.180572	3613.712719	24.212019
128.793650	3624.471410	24.217037
129.036270	3634.125145	24.222055
129.340979	3630.209302	24.227072
129.175525	3636.329330	24.232090
129.246641	3646.118174	24.237107
129.373717	3647.148937	24.242125
129.444361	3651.582809	24.247143
129.728797	3653.946364	24.252160
129.540256	3660.384834	24.257178
129.995980	3673.804222	24.262195
130.132520	3674.073866	24.267213
130.318778	3681.435860	24.272231
130.438261	3674.006092	24.277248
130.532923	3698.274948	24.282266
130.725621	3706.102487	24.287283
130.709373	3704.184523	24.292301
130.808300	3702.983419	24.297319
130.764349	3703.584957	24.302336
131.379863	3727.280156	24.307354
131.321612	3736.449440	24.312371
131.693311	3734.705859	24.317389
131.586496	3748.294835	24.322407
132.086728	3735.975727	24.327424
132.102639	3730.695664	24.332442
131.864565	3735.348018	24.337459
132.460330	3752.233756	24.342477
132.259478	3772.367990	24.347495
132.481903	3754.805523	24.352512
132.656662	3759.946307	24.357530
132.770165	3763.976602	24.362547
133.079282	3760.739622	24.367565
132.675977	3762.882759	24.372583
132.776545	3782.518219	24.377600
133.135959	3779.267001	24.382618
133.187989	3787.466345	24.387635
133.375062	3781.458614	24.392653
133.288044	3798.114482	24.397671
133.431593	3801.506649	24.402688
133.375897	3815.110845	24.407706
133.401385	3819.918436	24.412723
134.232092	3820.913437	24.417741
133.892202	3844.055076	24.422759
134.553706	3842.811616	24.427776
134.723069	3844.311445	24.432794
134.640408	3841.265709	24.437811
135.186242	3839.416110	24.442829
135.169209	3843.956692	24.447847
135.275018	3835.207264	24.452864
135.190225	3834.274791	24.457882
135.131337	3864.215040	24.462899
135.669545	3856.990311	24.467917
135.313648	3865.404105	24.472935
135.506342	3866.058216	24.477952
135.539167	3870.930760	24.482970
135.874134	3892.908615	24.487987
136.428298	3898.729656	24.493005
136.216681	3896.193522	24.498023
136.089797	3883.318971	24.503040
136.520397	3901.447359	24.508058
136.278492	3920.999908	24.513075
136.712577	3915.318609	24.518093
136.709300	3915.790174	24.523111
137.205646	3930.467818	24.528128
137.488665	3933.241163	24.533146
137.368073	3939.583444	24.538163
137.973705	3937.715271	24.543181
137.565734	3941.159798	24.548199
137.641101	3938.442264	24.553216
138.058835	3929.746668	24.558234
137.953501	3951.628974	24.563251
138.308705	3956.210338	24.568269
138.141533	3956.133360	24.573287
138.416799	3964.426172	24.578304
138.576472	3975.021948	24.583322
138.661251	3997.501286	24.588339
139.027615	3991.246040	24.593357
138.937977	4000.845151	24.598375
139.070937	3989.458443	24.603392
139.145490	4000.595183	24.608410
139.253106	4022.019428	24.613427
139.421714	4018.599721	24.618445
139.270647	4027.026153	24.623463
139.617607	4046.499478	24.628480
140.123664	4049.990370	24.633498
139.965035	4057.734496	24.638515
140.364556	4047.889696	24.643533
140.045977	4047.668465	24.648551
140.441635	4065.561058	24.653568
140.854652	4058.592436	24.658586
140.901586	4067.329471	24.663603
140.799383	4069.448392	24.668621
141.185575	4075.009861	24.673639
141.425341	4086.778471	24.678656
141.730411	4090.336512	24.683674
141.681803	4094.954847	24.688691
141.823693	4085.376336	24.693709
142.029569	4098.016849	24.698727
141.895207	4096.464905	24.703744
142.073859	4099.717053	24.708762
142.188898	4123.314580	24.713779
142.514208	4115.216171	24.718797
142.640456	4118.475423	24.723815
142.718463	4118.791781	24.728832
142.959582	4115.255306	24.733850
142.785891	4114.985673	24.738867
143.139873	4125.267444	24.743885
143.227369	4135.327943	24.748903
143.010246	4142.079266	24.753920
143.433011	4143.830922	24.758938
143.270497	4151.226072	24.763955
143.311226	4156.906193	24.768973
143.656819	4168.717984	24.773991
143.643244	4175.527763	24.779008
144.171030	4196.592871	24.784026
143.991827	4204.992555	24.789043
144.430184	4197.023445	24.794061
144.282968	4197.212497	24.799079
144.518155	4220.079922	24.804096
145.072367	4219.002255	24.809114
144.574996	4228.163410	24.814131
145.250272	4236.787849	24.819149
145.714573	4248.298896	24.824167
145.366890	4257.016315	24.829184
145.717493	4250.701362	24.834202
146.102590	4252.027695	24.839219
146.188469	4246.329112	24.844237
146.008691	4255.596785	24.849255
146.245985	4270.483020	24.854272
146.819874	4268.514537	24.859290
146.674260	4280.491216	24.864307
146.829152	4280.293186	24.869325
146.828874	4277.178597	24.874343
146.947418	4284.288654	24.879360
147.408525	4293.936945	24.884378
147.562474	4309.065402	24.889395
147.403757	4304.632707	24.894413
147.462901	4308.450449	24.899431
147.331015	4312.725880	24.904448
147.866807	4318.804497	24.909466
147.688637	4334.259666	24.914483
148.008885	4328.576591	24.919501
148.032841	4348.488089	24.924519
148.067522	4360.297947	24.929536
148.437861	4362.108710	24.934554
148.831719	4372.375380	24.939571
149.383388	4380.763624	24.944589
149.051423	4390.095949	24.949607
149.292254	4394.357735	24.954624
149.665190	4386.167035	24.959642
149.454568	4386.569773	24.964659
149.691731	4389.042863	24.969677
149.892859	4411.608275	24.974695
149.888281	4413.251152	24.979712
149.773540	4414.390912	24.984730
150.042175	4420.298800	24.989747
150.036537	4436.167318	24.994765
150.464007	4443.917768	24.999783
150.451304	4448.765740	25.004800
150.964920	4464.016724	25.009818
150.668699	4478.453589	25.014835
151.019533	4476.437743	25.019853
151.629995	4474.993201	25.024871
151.456425	4482.035152	25.029888
151.109532	4485.224754	25.034906
151.420272	4492.997704	25.039923
151.869960	4497.122559	25.044941
151.981282	4507.512486	25.049959
152.223926	4519.577852	25.054976
152.646207	4521.620240	25.059994
152.325896	4525.745785	25.065011
152.585789	4522.699120	25.070029
152.702076	4524.448794	25.075047
152.947705	4545.891858	25.080064
152.909500	4549.280809	25.085082
153.073336	4555.988139	25.090099
153.140486	4555.986557	25.095117
153.274498	4566.664949	25.100135
153.334567	4582.344749	25.105152
153.426476	4570.549377	25.110170
154.086944	4589.843103	25.115187
154.321298	4598.498214	25.120205
154.810284	4599.964103	25.125223
154.670441	4603.985761	25.130240
154.836878	4585.027820	25.135258
155.378738	4602.077765	25.140275
155.370924	4588.974219	25.145293
155.416843	4589.830650	25.150311
155.248648	4593.355327	25.155328
155.585051	4597.083134	25.160346
155.559547	4621.326847	25.165363
155.981906	4616.871892	25.170381
155.809085	4621.016360	25.175399
155.688612	4622.366573	25.180416
156.139809	4629.015334	25.185434
156.063946	4642.333763	25.190451
156.186961	4649.867739	25.195469
156.431525	4655.519020	25.200487
156.370080	4679.581333	25.205504
157.086882	4677.759255	25.210522
157.013840	4679.933284	25.215539
156.888680	4701.645076	25.220557
157.163308	4700.247452	25.225575
157.296227	4711.149003	25.230592
157.762702	4723.412163	25.235610
157.940694	4732.800449	25.240627
158.300460	4733.730151	25.245645
158.377885	4731.902086	25.250663
158.196592	4740.251208	25.255680
158.569647	4752.837007	25.260698
158.752270	4751.855481	25.265715
158.892128	4765.186342	25.270733
159.115137	4766.759287	25.275751
159.151893	4780.061551	25.280768
159.436356	4781.342375	25.285786
159.256516	4785.250991	25.290803
159.714041	4785.202107	25.295821
159.847839	4787.745928	25.300839
159.824569	4804.291105	25.305856
160.072438	4807.817828	25.310874
160.179007	4813.275430	25.315891
160.396723	4826.544624	25.320909
160.765647	4827.025478	25.325927
160.855935	4841.016715	25.330944
161.266540	4836.179312	25.335962
161.446423	4844.625420	25.340979
160.893035	4863.342328	25.345997
161.345298	4858.171968	25.351015
161.310803	4872.391810	25.356032
161.585685	4886.437584	25.361050
161.998466	4894.281262	25.366067
161.981756	4900.565777	25.371085
162.550248	4893.754555	25.376103
162.613235	4902.782373	25.381120
162.955280	4903.736284	25.386138
162.956060	4917.390363	25.391155
162.995615	4918.626688	25.396173
163.276802	4910.020894	25.401191
163.130497	4916.474933	25.406208
163.129737	4918.722874	25.411226
163.084097	4924.107267	25.416243
163.240885	4942.307396	25.421261
163.460344	4946.390943	25.426279
163.442777	4957.329392	25.431296
163.781280	4964.611261	25.436314
164.253510	4975.052008	25.441331
163.855679	4983.486724	25.446349
163.994154	4997.002303	25.451367
164.471758	5011.602946	25.456384
164.543855	5025.201995	25.461402
164.869107	5030.676237	25.466419
165.243266	5048.002519	25.471437
165.788269	5045.324395	25.476455
165.756482	5058.956423	25.481472
165.966839	5055.426408	25.486490
166.501074	5055.646779	25.491507
166.329738	5056.725859	25.496525
166.363015	5053.255089	25.501543
166.278253	5070.464416	25.506560
166.691065	5075.402800	25.511578
166.804141	5080.755458	25.516595
166.891660	5077.697846	25.521613
167.548768	5094.014913	25.526631
167.694865	5111.964195	25.531648
167.928151	5109.325853	25.536666
168.137914	5114.848384	25.541683
168.194140	5109.040199	25.546701
168.076510	5099.040941	25.551719
168.182056	5111.490173	25.556736
168.438188	5112.741062	25.561754
168.395166	5119.908961	25.566771
168.163279	5134.122339	25.571789
168.683196	5131.763387	25.576807
168.769525	5157.032168	25.581824
168.382997	5162.544748	25.586842
168.900383	5177.281513	25.591859
168.840793	5189.420271	25.596877
169.333780	5206.778249	25.601895
169.371770	5230.996635	25.606912
169.706163	5228.706188	25.611930
169.973642	5248.717123	25.616947
170.288282	5254.149883	25.621965
170.357287	5246.234308	25.626983
170.611932	5267.159418	25.632000
170.806351	5284.433021	25.637018
170.912903	5279.063005	25.642035
170.868625	5289.252383	25.647053
171.572265	5293.564599	25.652071
171.611363	5310.834016	25.657088
171.608948	5304.566063	25.662106
171.970537	5315.878315	25.667123
172.052250	5334.404000	25.672141
172.295132	5326.502129	25.677159
172.403444	5334.923334	25.682176
172.643778	5337.273974	25.687194
172.864344	5352.000974	25.692212
172.737298	5360.577720	25.697229
173.041519	5347.453389	25.702247
173.537864	5375.398616	25.707264
173.644379	5369.289025	25.712282
173.740147	5379.462364	25.717300
173.764140	5386.865807	25.722317
174.219609	5374.333101	25.727335
173.932147	5388.540155	25.732352
174.314532	5396.950674	25.737370
174.662711	5399.030651	25.742388
174.685823	5402.177293	25.747405
174.946345	5398.069466	25.752423
174.907057	5412.839543	25.757440
175.354349	5428.358417	25.762458
175.694078	5431.741697	25.767476
175.416078	5430.811184	25.772493
175.538695	5427.627192	25.777511
175.692568	5445.308571	25.782528
175.649614	5454.128203	25.787546
175.954594	5459.514590	25.792564
175.559012	5475.045460	25.797581
176.371474	5492.656453	25.802599
176.254923	5493.635131	25.807616
176.715668	5507.790096	25.812634
177.032526	5527.296234	25.817652
177.084252	5525.593624	25.822669
177.448372	5540.598686	25.827687
177.511593	5555.511808	25.832704
177.803068	5555.801520	25.837722
178.250606	5555.462092	25.842740
178.302536	5566.872259	25.847757
178.435647	5568.243579	25.852775
178.249112	5578.431491	25.857792
178.322569	5586.624682	25.862810
178.949452	5598.634355	25.867828
179.003853	5612.373883	25.872845
179.285348	5607.176422	25.877863
179.019085	5614.016841	25.882880
179.474795	5633.255178	25.887898
179.624522	5634.537903	25.892916
179.787995	5640.875582	25.897933
180.093624	5669.735812	25.902951
180.213440	5674.635469	25.907968
180.115917	5667.552190	25.912986
180.639699	5685.434872	25.918004
180.858750	5695.443873	25.923021
180.955734	5695.472796	25.928039
181.186116	5719.472630	25.933056
181.344879	5724.480846	25.938074
181.653481	5725.993251	25.943092
181.726365	5743.684434	25.948109
181.951916	5748.960415	25.953127
182.068324	5761.101980	25.958144
182.234789	5769.622480	25.963162
182.844761	5784.749322	25.968180
182.390130	5777.239942	25.973197
183.012389	5777.105507	25.978215
183.148988	5790.453528	25.983232
183.100350	5799.734261	25.988250
183.587969	5796.048704	25.993268
183.441541	5799.946523	25.998285
183.864431	5813.646488	26.003303
184.136776	5829.196297	26.008320
183.520881	5833.538087	26.013338
184.439126	5836.012073	26.018356
184.055817	5856.725382	26.023373
184.447203	5855.367403	26.028391
184.743144	5866.804338	26.033408
184.657145	5888.112741	26.038426
185.386083	5878.629714	26.043444
185.296884	5904.946355	26.048461
185.648974	5913.439353	26.053479
185.784375	5902.401355	26.058496
186.001188	5920.286291	26.063514
186.418102	5924.676083	26.068532
186.603466	5943.394830	26.073549
186.792747	5935.247916	26.078567
186.603327	5946.437609	26.083584
186.561738	5939.284301	26.088602
187.003448	5955.001526	26.093620
187.258395	5967.678739	26.098637
187.318758	5976.702093	26.103655
187.372418	5980.543203	26.108672
187.119177	6000.869710	26.113690
187.910904	6002.046971	26.118708
188.131451	6021.627950	26.123725
188.390826	6033.830331	26.128743
188.707297	6030.310102	26.133760
188.394284	6035.258685	26.138778
188.913143	6050.255156	26.143796
188.740255	6061.319323	26.148813
188.944760	6058.072816	26.153831
189.202589	6074.697232	26.158848
189.401249	6083.661521	26.163866
189.719823	6098.688833	26.168884
189.405745	6123.942746	26.173901
190.169746	6129.595206	26.178919
190.604890	6138.657425	26.183936
190.647408	6144.200918	26.188954
190.826769	6138.627164	26.193972
191.176223	6155.766574	26.198989
191.085498	6168.092392	26.204007
191.297600	6168.358240	26.209024
191.206449	6178.452770	26.214042
191.832820	6183.644427	26.219060
191.859970	6203.045773	26.224077
192.351123	6214.657005	26.229095
192.764011	6226.449756	26.234112
193.036713	6229.975841	26.239130
193.397365	6230.794436	26.244148
192.831408	6230.527476	26.249165
193.647458	6231.644021	26.254183
193.516716	6225.982949	26.259200
193.954818	6236.647576	26.264218
194.147721	6242.679748	26.269236
194.271268	6242.260835	26.274253
194.292342	6237.633999	26.279271
194.579459	6242.651849	26.284288
194.464743	6269.274197	26.289306
194.912476	6264.552304	26.294324
194.896275	6272.139246	26.299341
195.025847	6286.082728	26.304359
195.399729	6291.789593	26.309376
195.220764	6304.542848	26.314394
195.615528	6311.368651	26.319412
195.673079	6334.085820	26.324429
195.765721	6337.350311	26.329447
196.212025	6348.540588	26.334464
196.431047	6359.904763	26.339482
196.564748	6359.603100	26.344500
196.627161	6383.264707	26.349517
196.828935	6389.281288	26.354535
197.522402	6396.390065	26.359552
197.425526	6420.747596	26.364570
197.803130	6420.504799	26.369588
197.811618	6426.956667	26.374605
197.865568	6441.549224	26.379623
198.287985	6441.321850	26.384640
198.309964	6455.776360	26.389658
198.682890	6456.871764	26.394676
199.124532	6478.652841	26.399693
198.721371	6480.178395	26.404711
199.241550	6492.104812	26.409728
199.141592	6507.868152	26.414746
199.551314	6510.899815	26.419764
199.722802	6521.584355	26.424781
199.943528	6529.094390	26.429799
200.212667	6537.876349	26.434816
199.824637	6535.169711	26.439834
200.020778	6557.238860	26.444852
200.328397	6561.090055	26.449869
200.300126	6586.964531	26.454887
200.785806	6588.849412	26.459904
200.858417	6613.999917	26.464922
201.348232	6620.647863	26.469940
201.560615	6632.492227	26.474957
201.800228	6655.972887	26.479975
202.302218	6652.328080	26.484992
202.228885	6668.017070	26.490010
202.544532	6676.491309	26.495028
202.775623	6683.004100	26.500045
203.389017	6686.828336	26.505063
203.396836	6691.259288	26.510080
203.252769	6702.898848	26.515098
203.701429	6696.967617	26.520116
203.856991	6710.693714	26.525133
203.811857	6727.601332	26.530151
204.349292	6732.423518	26.535168
204.343494	6744.541959	26.540186
204.614421	6756.219192	26.545204
204.928490	6758.301851	26.550221
205.242468	6769.631696	26.555239
205.418502	6781.106474	26.560256
205.371103	6791.857363	26.565274
205.566582	6787.294440	26.570292
205.762929	6796.117737	26.575309
206.070878	6808.913665	26.580327
206.740166	6811.806323	26.585344
206.603700	6825.669082	26.590362
206.997599	6840.877609	26.595380
207.236403	6851.054210	26.600397
206.812637	6844.938893	26.605415
207.366378	6857.828863	26.610432
207.317052	6876.930989	26.615450
207.684647	6878.621997	26.620468
207.684149	6893.898228	26.625485
207.685915	6919.644609	26.630503
207.902096	6923.191235	26.635520
208.384913	6943.030039	26.640538
208.788636	6956.784584	26.645556
208.952490	6963.707972	26.650573
208.924385	6979.261390	26.655591
209.479085	6990.710654	26.660608
209.531218	7006.303590	26.665626
210.020343	6997.416493	26.670644
209.968389	7024.334545	26.675661
210.137085	7036.069080	26.680679
210.419337	7036.355627	26.685696
210.320159	7055.402418	26.690714
210.832769	7061.593075	26.695732
210.789062	7081.290001	26.700749
210.789887	7109.902422	26.705767
211.567915	7101.480222	26.710784
211.630968	7131.693188	26.715802
211.861716	7130.754754	26.720820
212.187166	7146.137168	26.725837
212.044178	7154.692314	26.730855
212.557456	7162.116412	26.735872
212.685142	7177.181863	26.740890
212.916922	7182.672333	26.745908
213.348322	7190.944944	26.750925
213.166778	7217.326307	26.755943
213.806115	7213.862649	26.760960
213.799556	7223.619311	26.765978
213.755628	7230.705606	26.770996
214.489801	7234.736051	26.776013
214.407391	7250.107315	26.781031
214.462797	7249.717775	26.786048
214.635215	7270.843468	26.791066
214.279066	7278.270552	26.796084
215.009723	7305.690463	26.801101
215.025742	7311.760989	26.806119
215.305864	7328.072682	26.811136
215.570341	7346.194734	26.816154
215.752928	7361.342644	26.821172
216.267611	7367.294408	26.826189
216.127253	7380.329640	26.831207
216.891267	7390.462178	26.836224
216.778591	7407.262756	26.841242
217.306206	7405.930940	26.846260
217.861969	7421.084084	26.851277
217.637101	7431.116472	26.856295
217.982288	7440.744934	26.861312
218.173680	7457.418034	26.866330
218.266798	7455.027008	26.871348
218.348149	7462.953621	26.876365
218.437211	7483.489231	26.881383
218.738592	7495.566057	26.886400
218.787960	7510.239911	26.891418
219.192420	7528.829736	26.896436
219.853505	7535.600169	26.901453
220.025309	7548.074219	26.906471
220.368345	7551.379432	26.911488
220.271573	7575.722170	26.916506
220.654999	7576.163700	26.921524
220.706229	7583.543967	26.926541
220.968847	7599.540603	26.931559
221.317152	7604.614927	26.936576
221.521093	7613.148334	26.941594
221.732038	7635.682854	26.946612
221.942942	7631.110048	26.951629
222.113521	7647.202315	26.956647
222.430968	7660.518034	26.961664
222.354471	7667.244417	26.966682
222.468719	7691.814707	26.971700
222.917991	7691.106313	26.976717
223.079913	7705.293027	26.981735
223.356997	7720.953402	26.986752
223.453024	7734.776889	26.991770
223.874384	7750.631605	26.996788
223.957145	7759.463214	27.001805
224.146395	7780.352059	27.006823
224.319515	7783.168707	27.011840
224.438769	7810.224376	27.016858
224.656461	7817.428317	27.021876
224.880190	7831.465486	27.026893
225.251637	7853.590126	27.031911
225.436889	7861.361099	27.036928
226.193365	7882.658743	27.041946
226.171720	7887.784160	27.046964
226.391223	7891.128011	27.051981
226.577157	7910.652458	27.056999
226.807035	7910.263954	27.062016
227.474152	7925.840272	27.067034
227.272628	7939.160999	27.072052
227.646576	7937.686796	27.077069
227.666130	7954.865435	27.082087
227.947543	7962.700099	27.087104
228.120782	7976.370799	27.092122
228.660949	7991.715337	27.097140
228.811159	8003.679723	27.102157
228.860197	8018.699123	27.107175
228.684134	8008.784110	27.112192
229.188612	8028.500165	27.117210
229.348350	8039.932861	27.122228
229.823088	8047.176278	27.127245
229.833101	8069.862045	27.132263
229.862935	8061.237085	27.137280
230.132068	8083.368742	27.142298
230.271044	8100.049616	27.147316
230.558710	8114.559330	27.152333
231.047494	8135.688153	27.157351
231.290396	8138.270385	27.162368
231.576739	8152.071394	27.167386
231.431202	8158.232005	27.172404
232.012375	8165.803672	27.177421
232.025069	8187.144502	27.182439
232.199502	8186.865212	27.187456
232.471652	8217.697865	27.192474
232.498294	8219.183935	27.197492
232.736504	8239.747032	27.202509
233.051464	8254.943987	27.207527
233.473257	8269.541134	27.212544
233.816986	8291.977402	27.217562
233.863540	8312.201293	27.222580
234.242495	8322.181547	27.227597
234.593692	8332.985652	27.232615
234.571587	8334.809078	27.237632
235.234088	8359.186444	27.242650
235.222846	8379.394781	27.247668
235.516950	8374.094297	27.252685
235.472706	8399.551339	27.257703
235.525040	8410.061514	27.262720
235.982893	8421.337213	27.267738
235.908199	8442.105978	27.272756
236.553916	8457.396471	27.277773
236.947934	8477.169179	27.282791
237.191810	8501.945341	27.287808
237.355876	8502.197130	27.292826
237.417330	8519.667996	27.297844
237.995941	8525.879029	27.302861
237.991510	8551.591256	27.307879
238.428991	8559.540600	27.312896
238.962764	8568.001802	27.317914
238.988489	8593.095444	27.322932
239.233543	8586.682037	27.327949
239.139276	8613.448281	27.332967
239.569862	8627.852877	27.337984
239.918624	8627.339119	27.343002
240.174464	8647.101038	27.348020
240.281555	8643.215511	27.353037
240.493543	8670.281706	27.358055
240.769715	8672.025860	27.363072
241.235002	8690.761375	27.368090
241.060218	8712.772024	27.373108
241.926359	8716.988981	27.378125
242.006288	8744.351302	27.383143
242.033729	8740.952382	27.388160
242.387955	8742.396090	27.393178
242.343632	8755.185729	27.398196
242.898088	8753.587043	27.403213
243.027821	8777.895691	27.408231
243.491867	8786.213363	27.413248
244.121528	8783.040091	27.418266
243.940441	8799.892055	27.423284
244.361962	8811.426919	27.428301
244.384428	8817.006173	27.433319
244.877982	8814.825952	27.438336
245.061349	8829.642691	27.443354
245.208045	8839.760188	27.448372
245.453416	8840.071787	27.453389
245.447646	8838.082930	27.458407
245.962027	8847.829188	27.463424
246.116880	8857.098497	27.468442
246.041237	8866.511527	27.473460
246.252958	8876.250396	27.478477
246.868996	8896.771489	27.483495
246.625285	8897.254643	27.488512
247.216521	8907.241876	27.493530
246.994286	8932.087985	27.498548
247.612867	8931.976220	27.503565
247.642002	8953.345284	27.508583
247.696952	8964.373743	27.513600
248.112441	8980.427601	27.518618
248.312393	8989.300362	27.523636
248.396735	9010.941599	27.528653
248.579252	9021.136785	27.533671
248.975640	9041.837800	27.538688
249.085558	9066.606288	27.543706
249.136566	9089.202421	27.548724
250.031348	9100.916756	27.553741
249.929732	9117.391944	27.558759
250.195388	9132.216612	27.563776
250.534977	9150.268411	27.568794
250.677752	9177.045988	27.573812
251.094973	9185.851380	27.578829
251.299935	9204.881895	27.583847
251.630892	9221.310793	27.588864
251.779317	9229.618709	27.593882
251.810722	9253.463805	27.598900
252.316631	9274.158020	27.603917
252.781050	9295.058441	27.608935
253.297395	9305.378164	27.613952
254.264622	9307.108046	27.618970
254.295441	9338.077341	27.623988
254.603441	9335.749728	27.629005
254.850245	9326.077438	27.634023
255.086209	9332.990709	27.639040
255.111143	9327.320093	27.644058
255.024172	9341.263493	27.649076
255.554935	9362.357845	27.654093
255.439537	9361.507311	27.659111
255.724058	9374.934690	27.664128
256.094197	9383.483288	27.669146
256.373424	9399.339541	27.674164
256.466360	9412.281873	27.679181
256.869048	9413.715260	27.684199
257.074384	9441.303803	27.689216
257.396208	9453.845107	27.694234
257.263972	9454.205045	27.699252
257.560032	9470.935400	27.704269
257.777537	9493.354859	27.709287
257.905273	9508.081385	27.714304
258.047946	9516.480211	27.719322
258.227101	9542.017106	27.724340
259.030063	9562.326919	27.729357
259.293298	9576.364598	27.734375
259.630937	9589.248447	27.739392
260.471387	9592.572592	27.744410
260.362768	9612.295981	27.749428
260.580734	9622.992241	27.754445
260.987947	9625.579033	27.759463
260.603108	9638.763709	27.764480
261.077405	9652.724764	27.769498
261.343027	9669.545448	27.774516
261.693539	9683.072455	27.779533
261.858516	9685.497676	27.784551
262.053430	9702.508930	27.789568
262.537849	9713.929258	27.794586
262.223087	9731.072967	27.799604
263.275720	9742.552092	27.804621
263.328090	9755.579409	27.809639
263.244860	9759.371612	27.814656
263.625323	9769.567597	27.819674
263.694072	9789.109796	27.824692
263.954658	9805.095586	27.829709
264.136522	9816.786657	27.834727
264.244671	9834.980743	27.839744
264.524404	9849.771445	27.844762
264.800133	9873.028698	27.849780
265.357695	9888.736946	27.854797
265.693074	9897.709905	27.859815
265.621345	9924.678647	27.864832
266.126316	9937.267219	27.869850
265.971442	9962.806503	27.874868
266.540710	9973.572472	27.879885
267.017191	9995.440831	27.884903
267.323491	10009.471761	27.889920
267.613590	10021.513766	27.894938
267.509137	10044.990188	27.899956
267.819519	10061.471411	27.904973
268.445901	10066.441410	27.909991
268.682835	10095.413995	27.915008
269.075711	10100.728334	27.920026
269.271658	10123.223146	27.925044
269.395330	10132.291155	27.930061
270.045264	10150.822919	27.935079
270.259659	10160.555037	27.940096
270.349209	10167.770222	27.945114
270.727770	10192.221812	27.950132
271.013170	10201.961109	27.955149
271.619944	10215.555656	27.960167
271.867146	10219.226305	27.965184
272.232448	10225.726213	27.970202
272.268674	10248.190913	27.975220
272.286048	10243.267306	27.980237
272.675576	10258.782351	27.985255
272.884765	10280.884425	27.990272
273.444721	10294.285890	27.995290
273.440085	10311.679046	28.000308
273.422540	10320.814656	28.005325
274.003366	10333.131785	28.010343
273.679967	10349.741060	28.015360
273.967719	10371.591538	28.020378
274.285028	10404.451976	28.025396
274.511115	10416.460754	28.030413
274.912686	10436.919270	28.035431
275.097594	10470.874803	28.040448
275.759902	10480.124868	28.045466
276.107009	10497.099166	28.050484
276.531441	10509.144512	28.055501
277.021618	10527.891453	28.060519
276.819863	10544.033294	28.065536
277.658000	10555.789598	28.070554
277.502856	10558.062312	28.075572
277.810785	10579.726163	28.080589
278.305894	10581.093940	28.085607
278.276276	10597.171099	28.090624
278.897217	10616.679624	28.095642
279.171096	10632.705006	28.100660
279.447106	10635.429497	28.105677
279.523135	10649.869394	28.110695
279.391886	10669.972053	28.115712
279.779181	10681.702231	28.120730
280.138606	10704.646659	28.125748
280.323629	10716.854696	28.130765
280.726365	10733.812157	28.135783
280.695281	10751.629305	28.140800
281.309920	10760.075928	28.145818
281.562361	10775.175325	28.150836
281.711998	10792.080200	28.155853
282.130245	10804.725567	28.160871
281.944722	10826.001863	28.165888
282.539436	10836.826444	28.170906
282.999457	10851.729254	28.175924
283.217160	10882.535071	28.180941
283.396894	10894.608605	28.185959
283.805243	10915.542479	28.190976
283.993627	10926.182262	28.195994
284.415906	10943.918274	28.201012
284.449380	10961.605211	28.206029
285.025129	10962.647678	28.211047
284.939454	10987.396347	28.216064
285.459188	11004.886237	28.221082
285.613409	11026.201104	28.226100
285.925108	11045.055403	28.231117
286.427500	11069.958977	28.236135
286.595457	11080.855939	28.241152
286.970446	11098.308436	28.246170
287.177927	11118.390249	28.251188
287.207113	11139.697599	28.256205
288.105759	11150.984206	28.261223
288.353950	11167.263341	28.266240
289.007925	11176.907555	28.271258
288.965819	11197.675265	28.276276
289.367889	11201.442628	28.281293
289.664444	11207.598981	28.286311
289.519900	11217.616485	28.291328
290.254912	11240.066172	28.296346
290.301713	11251.632519	28.301364
290.353336	11276.039021	28.306381
290.740348	11284.881301	28.311399
290.616228	11302.162934	28.316416
291.652031	11324.865499	28.321434
291.786788	11342.425782	28.326452
291.604366	11363.146021	28.331469
292.329512	11378.174042	28.336487
292.618574	11398.249003	28.341504
292.657018	11414.325162	28.346522
293.402926	11437.714063	28.351540
293.497845	11452.162581	28.356557
294.179384	11465.642600	28.361575
294.138494	11484.086189	28.366592
294.476810	11502.287390	28.371610
294.667952	11513.563724	28.376628
294.830360	11532.243177	28.381645
295.390994	11536.414566	28.386663
295.540263	11568.287223	28.391680
296.035653	11566.910003	28.396698
296.195066	11577.017664	28.401716
296.465251	11601.561817	28.406733
296.961735	11611.163026	28.411751
297.091684	11625.941546	28.416768
297.572121	11640.673097	28.421786
297.568183	11653.332284	28.426804
297.573403	11673.701970	28.431821
298.235580	11685.844367	28.436839
298.641046	11718.877257	28.441856
298.981382	11715.005966	28.446874
299.352091	11748.739604	28.451892
299.493443	11756.477187	28.456909
299.765362	11772.327534	28.461927
299.649618	11786.982984	28.466944
299.950304	11809.292619	28.471962
300.312181	11820.915952	28.476980
300.718958	11844.776020	28.481997
301.286760	11850.908208	28.487015
301.223620	11875.879845	28.492032
301.499258	11882.582003	28.497050
302.063268	11892.386517	28.502068
302.062877	11907.826655	28.507085
302.437051	11926.567637	28.512103
302.772306	11953.909689	28.517120
302.949063	11967.968495	28.522138
303.298573	11990.505098	28.527156
303.435039	12001.973620	28.532173
303.956018	12021.341234	28.537191
304.402985	12044.121795	28.542208
304.677391	12069.488550	28.547226
305.395924	12076.873888	28.552244
305.270337	12096.044473	28.557261
305.732636	12098.959001	28.562279
306.141224	12124.571526	28.567296
306.400655	12135.375266	28.572314
306.915805	12145.522102	28.577332
307.142285	12164.678618	28.582349
307.271309	12184.390232	28.587367
307.615828	12196.752635	28.592384
307.961774	12221.505808	28.597402
308.322658	12231.941402	28.602420
308.463274	12259.194844	28.607437
308.637175	12264.158487	28.612455
309.062674	12284.308092	28.617472
309.412360	12311.233905	28.622490
309.864414	12327.289784	28.627508
309.862481	12352.422215	28.632525
309.856001	12354.702087	28.637543
310.051026	12392.423165	28.642560
310.386250	12412.802191	28.647578
311.190021	12438.346650	28.652596
311.330292	12456.053784	28.657613
311.948087	12479.558379	28.662631
312.054008	12499.740661	28.667648
312.572522	12518.888654	28.672666
313.045505	12538.264832	28.677684
313.074661	12565.225209	28.682701
313.487717	12573.543841	28.687719
313.581099	12605.371052	28.692736
313.833302	12608.914563	28.697754
314.225964	12621.910714	28.702772
314.516061	12653.431252	28.707789
315.112791	12669.532864	28.712807
315.305522	12687.872960	28.717824
315.674910	12719.029075	28.722842
316.078913	12726.362764	28.727860
316.063544	12749.466683	28.732877
316.558530	12771.181304	28.737895
317.058982	12783.176372	28.742912
317.380972	12808.757033	28.747930
317.985698	12816.917993	28.752948
318.039163	12844.306610	28.757965
318.312490	12852.314418	28.762983
318.562788	12871.067540	28.768000
318.827716	12897.398470	28.773018
319.161617	12906.857164	28.778036
319.260691	12932.783798	28.783053
319.753864	12944.627326	28.788071
320.148808	12959.465633	28.793088
320.407867	12985.737793	28.798106
320.664797	12987.091630	28.803124
321.253016	13019.802219	28.808141
321.625556	13026.532941	28.813159
321.754428	13043.935293	28.818176
321.885098	13058.771732	28.823194
322.364804	13070.882339	28.828212
322.505535	13096.862226	28.833229
322.898961	13102.654986	28.838247
323.081174	13129.750133	28.843264
323.524223	13143.195387	28.848282
323.830574	13157.629337	28.853300
323.881238	13177.593092	28.858317
324.422447	13198.391308	28.863335
324.396948	13228.048833	28.868352
324.986616	13241.632224	28.873370
324.941800	13262.497576	28.878388
325.275319	13281.508462	28.883405
325.770402	13311.434565	28.888423
326.314092	13332.481545	28.893440
326.128627	13362.715804	28.898458
326.789438	13386.856014	28.903476
327.060301	13415.730422	28.908493
327.599986	13442.053003	28.913511
328.118699	13458.254991	28.918528
328.208440	13482.340146	28.923546
328.884962	13506.356582	28.928564
329.215010	13524.722172	28.933581
329.614718	13540.371856	28.938599
330.027916	13562.291766	28.943616
329.933857	13591.557843	28.948634
330.486903	13593.173193	28.953652
330.656535	13616.955339	28.958669
331.210156	13637.213072	28.963687
331.621972	13659.313005	28.968704
331.761480	13671.965777	28.973722
332.094237	13702.069185	28.978740
332.264925	13727.131033	28.983757
332.615555	13739.591313	28.988775
333.036480	13755.411053	28.993792
332.999839	13781.638876	28.998810
333.766677	13800.301269	29.003828
333.829515	13838.607055	29.008845
334.216822	13859.469413	29.013863
334.888105	13884.105074	29.018880
335.082715	13906.031681	29.023898
335.584522	13932.851468	29.028916
336.042311	13947.844183	29.033933
336.338968	13974.124319	29.038951
336.705502	13983.609759	29.043968
336.933025	14011.806820	29.048986
337.630651	14021.013686	29.054004
337.770074	14040.520937	29.059021
337.862459	14055.172340	29.064039
338.197867	14071.841842	29.069056
338.711877	14092.021590	29.074074
339.215823	14111.938254	29.079092
339.429633	14132.290670	29.084109
339.718944	14145.401285	29.089127
340.014163	14168.752100	29.094144
340.096905	14186.341397	29.099162
340.574081	14213.400553	29.104180
340.930717	14232.779095	29.109197
340.973706	14252.386090	29.114215
341.453529	14274.798693	29.119232
341.558435	14300.069313	29.124250
342.060999	14312.657763	29.129268
342.385950	14346.303487	29.134285
342.958716	14369.920713	29.139303
343.468357	14391.625613	29.144320
343.454943	14420.723791	29.149338
343.569264	14437.009446	29.154356
343.985967	14464.386361	29.159373
344.305747	14474.046890	29.164391
344.511415	14502.267326	29.169408
345.065126	14524.059673	29.174426
345.623913	14547.119958	29.179444
345.836075	14570.622212	29.184461
346.311958	14588.469970	29.189479
346.818792	14601.009077	29.194496
346.792479	14629.658997	29.199514
347.040009	14648.197118	29.204532
347.342908	14674.166853	29.209549
347.780103	14685.864882	29.214567
348.037374	14714.915627	29.219584
348.332802	14746.770304	29.224602
348.930140	14759.419066	29.229620
349.423586	14791.614592	29.234637
349.418859	14817.466825	29.239655
350.122680	14834.641953	29.244672
349.875264	14875.537476	29.249690
350.858632	14891.402349	29.254708
350.932929	14922.595745	29.259725
351.238183	14951.246512	29.264743
351.922469	14963.963000	29.269760
352.125669	14995.778260	29.274778
352.568724	15006.295028	29.279796
352.814550	15033.984880	29.284813
353.100894	15070.180780	29.289831
353.707999	15088.529066	29.294848
353.911195	15114.596383	29.299866
354.582790	15120.967979	29.304884
354.850021	15148.380232	29.309901
355.081238	15182.536517	29.314919
355.746993	15199.522886	29.319936
355.950641	15228.428952	29.324954
356.698016	15232.116474	29.329972
356.832585	15258.365601	29.334989
356.950888	15267.992171	29.340007
357.327170	15292.048319	29.345024
357.507943	15321.387049	29.350042
358.081587	15341.035184	29.355060
358.401073	15373.735069	29.360077
358.651281	15393.361142	29.365095
359.018146	15409.137840	29.370112
359.456470	15435.007556	29.375130
359.735909	15459.291184	29.380148
360.190709	15484.992753	29.385165
360.484560	15516.072126	29.390183
360.982471	15529.079972	29.395200
361.504869	15564.172393	29.400218
361.706786	15584.514393	29.405236
362.162062	15604.064219	29.410253
362.138225	15620.645017	29.415271
362.610797	15644.542311	29.420288
362.871355	15676.166554	29.425306
363.431402	15705.249323	29.430324
363.879077	15735.203465	29.435341
364.105260	15760.851884	29.440359
364.427605	15779.481352	29.445376
364.833782	15799.376845	29.450394
365.365967	15827.015907	29.455412
365.435924	15841.283291	29.460429
365.590922	15879.299588	29.465447
366.202027	15889.897870	29.470464
366.657078	15923.244724	29.475482
366.732348	15941.779713	29.480500
367.694166	15965.495622	29.485517
367.684127	15991.560212	29.490535
367.966988	16017.078279	29.495552
368.233046	16036.385673	29.500570
368.839985	16053.951682	29.505588
369.286731	16070.940527	29.510605
369.214726	16095.718298	29.515623
369.903483	16116.970255	29.520640
369.883174	16145.798354	29.525658
370.592565	16170.502080	29.530676
371.022212	16197.410020	29.535693
371.334142	16215.363920	29.540711
371.751370	16238.697483	29.545728
372.042026	16264.892430	29.550746
372.598978	16284.315900	29.555764
373.020264	16305.664385	29.560781
373.141570	16326.915954	29.565799
373.782917	16341.644044	29.570816
374.040457	16366.033513	29.575834
374.212685	16395.232126	29.580852
374.577318	16416.203946	29.585869
374.869562	16449.440098	29.590887
375.573104	16474.720587	29.595904
375.714705	16513.374219	29.600922
376.082656	16530.124375	29.605940
376.513647	16559.496401	29.610957
376.669964	16598.091050	29.615975
377.308162	16615.851097	29.620992
377.476974	16648.472835	29.626010
377.969124	16668.528540	29.631028
378.515183	16701.606545	29.636045
378.812953	16729.199221	29.641063
379.251390	16762.178513	29.646080
379.830073	16794.943928	29.651098
379.827143	16811.517729	29.656116
380.460315	16840.911964	29.661133
380.600487	16870.540747	29.666151
381.408339	16898.263662	29.671168
381.259094	16921.047231	29.676186
381.926787	16945.336569	29.681204
382.171875	16960.778662	29.686221
382.381790	17008.716106	29.691239
383.109519	17025.074616	29.696256
383.130165	17066.236992	29.701274
383.545636	17094.997770	29.706292
384.081548	17120.283347	29.711309
384.049922	17148.821864	29.716327
384.926048	17182.386886	29.721344
385.081115	17222.888987	29.726362
385.447544	17253.015386	29.731380
386.238584	17276.651107	29.736397
386.523519	17319.395583	29.741415
386.903742	17333.425317	29.746432
387.168821	17369.941892	29.751450
387.617553	17386.077378	29.756468
388.316943	17416.932419	29.761485
388.591677	17449.700566	29.766503
389.404914	17467.724189	29.771520
389.461766	17488.907520	29.776538
389.638282	17519.795692	29.781556
390.619562	17539.982737	29.786573
390.558488	17571.224024	29.791591
391.191180	17592.449329	29.796608
391.512574	17622.681588	29.801626
392.085054	17640.754705	29.806644
392.356176	17662.528618	29.811661
392.493745	17692.438317	29.816679
392.902157	17715.933061	29.821696
393.121077	17741.131749	29.826714
393.673212	17767.962069	29.831732
394.030878	17791.077525	29.836749
394.186465	17817.688226	29.841767
394.601415	17837.523242	29.846784
394.935914	17866.306641	29.851802
395.489544	17892.640348	29.856820
395.976036	17923.271459	29.861837
395.891970	17950.152190	29.866855
396.686822	17964.408627	29.871872
396.905323	18004.809125	29.876890
396.779716	18013.676841	29.881908
397.310997	18048.445168	29.886925
397.260238	18088.534160	29.891943
398.069465	18116.698712	29.896960
398.607348	18161.947841	29.901978
399.286753	18193.558015	29.906996
399.652108	18219.281791	29.912013
400.235658	18253.903171	29.917031
400.764766	18282.700799	29.922048
400.738396	18307.274104	29.927066
400.796982	18345.036125	29.932084
401.192507	18373.050453	29.937101
401.431330	18421.706043	29.942119
402.238784	18450.188321	29.947136
402.982602	18477.820433	29.952154
403.811288	18510.462731	29.957172
403.957809	18543.785518	29.962189
404.315065	18584.195985	29.967207
404.909339	18601.475154	29.972224
405.266024	18628.034949	29.977242
405.802030	18653.926637	29.982260
406.291496	18680.740424	29.987277
406.312002	18711.724413	29.992295
406.919611	18733.128742	29.997312
407.339158	18765.568097	30.002330
407.641875	18801.107312	30.007348
408.096331	18825.295964	30.012365
408.261118	18853.347708	30.017383
408.803469	18882.122110	30.022400
409.335241	18916.045587	30.027418
409.585772	18944.583045	30.032436
409.989492	18978.133715	30.037453
410.237932	19014.320850	30.042471
411.013138	19041.489939	30.047488
411.189224	19075.307070	30.052506
411.508335	19100.899549	30.057524
412.097914	19127.571365	30.062541
412.315627	19171.280779	30.067559
412.890084	19199.908528	30.072576
413.339278	19230.332230	30.077594
413.570924	19260.771495	30.082612
414.290313	19288.375888	30.087629
414.665193	19327.880303	30.092647
414.902985	19353.491356	30.097664
415.524609	19386.510172	30.102682
415.630329	19414.788619	30.107700
416.654417	19443.153188	30.112717
416.865005	19470.465290	30.117735
417.384247	19492.375527	30.122752
418.044833	19515.816887	30.127770
418.099912	19557.944559	30.132788
418.845292	19578.519975	30.137805
419.248090	19608.701369	30.142823
419.211277	19627.815539	30.147840
419.802098	19654.087542	30.152858
419.981315	19690.057414	30.157876
420.516453	19706.617564	30.162893
420.928391	19750.159182	30.167911
421.184522	19774.720995	30.172928
421.616081	19798.456060	30.177946
421.550611	19831.387661	30.182964
422.138309	19854.403267	30.187981
422.376099	19891.716591	30.192999
422.717217	19920.001077	30.198016
423.212190	19960.789377	30.203034
423.509041	19999.184172	30.208052
424.311182	20025.320883	30.213069
424.650267	20085.013564	30.218087
425.107471	20105.911651	30.223104
425.743887	20141.218750	30.228122
425.771042	20179.898236	30.233140
426.450662	20201.595243	30.238157
426.934540	20231.368607	30.243175
426.949761	20264.927812	30.248192
427.466367	20300.961403	30.253210
427.699871	20339.980769	30.258228
428.490129	20374.072538	30.263245
428.701292	20421.981725	30.268263
429.189062	20452.268822	30.273280
429.568945	20496.088860	30.278298
430.060677	20538.939780	30.283316
430.656645	20583.077455	30.288333
430.991106	20619.554956	30.293351
431.448636	20647.986951	30.298368
431.986882	20686.937768	30.303386
432.397733	20720.971627	30.308404
433.169112	20757.299864	30.313421
433.548229	20796.373447	30.318439
433.848764	20824.256233	30.323456
434.537913	20849.328174	30.328474
434.947386	20888.660253	30.333492
435.130718	20925.623819	30.338509
435.705327	20960.066227	30.343527
436.044286	20991.186188	30.348544
436.786147	21035.458574	30.353562
436.917788	21070.414413	30.358580
437.438524	21102.639723	30.363597
437.891008	21143.545138	30.368615
438.381407	21174.213086	30.373632
438.893438	21200.912072	30.378650
439.195214	21241.331809	30.383668
439.934848	21281.639763	30.388685
440.037204	21314.082926	30.393703
440.408728	21345.644365	30.398720
440.879539	21383.119520	30.403738
441.482662	21423.198126	30.408756
442.248351	21448.849570	30.413773
443.209499	21479.851700	30.418791
443.026225	21516.672252	30.423808
443.466862	21540.665283	30.428826
443.742859	21582.072414	30.433844
444.638709	21622.886697	30.438861
444.777979	21641.013763	30.443879
445.176369	21677.973343	30.448896
445.401816	21707.478309	30.453914
445.802449	21746.323475	30.458932
446.461912	21782.043313	30.463949
446.985564	21820.940824	30.468967
447.264706	21852.308786	30.473984
448.034448	21884.183757	30.479002
448.221435	21916.915235	30.484020
448.425214	21939.566769	30.489037
448.908259	21987.347100	30.494055
449.504932	22018.520912	30.499072
450.373478	22042.820697	30.504090
450.673174	22084.507380	30.509108
450.866918	22107.644877	30.514125
451.621935	22145.531961	30.519143
451.942601	22164.570920	30.524160
452.499769	22194.002916	30.529178
452.616453	22224.755115	30.534196
453.159043	22248.111016	30.539213
453.543743	22282.961254	30.544231
453.700167	22309.517432	30.549248
454.032640	22338.359289	30.554266
454.532516	22377.468577	30.559284
455.100742	22417.366095	30.564301
455.365848	22460.262545	30.569319
456.003285	22498.206143	30.574336
456.494752	22521.417929	30.579354
456.462056	22568.853192	30.584372
457.118097	22609.824652	30.589389
457.583689	22655.922529	30.594407
458.066692	22701.408985	30.599424
458.766202	22735.104257	30.604442
458.983285	22786.753154	30.609460
459.578283	22819.401507	30.614477
459.981002	22861.222849	30.619495
460.585692	22904.158835	30.624512
460.814447	22938.448050	30.629530
461.125874	22989.438584	30.634548
461.693677	23019.609811	30.639565
462.003750	23068.812621	30.644583
462.529229	23125.824970	30.649600
463.415353	23163.929168	30.654618
463.560963	23213.927561	30.659636
463.994978	23244.838818	30.664653
464.356286	23299.007371	30.669671
465.082852	23344.567201	30.674688
465.701031	23387.420174	30.679706
466.162555	23435.559791	30.684724
466.613007	23487.031845	30.689741
467.035701	23521.663871	30.694759
467.506831	23565.177128	30.699776
468.228881	23595.833202	30.704794
468.589130	23651.461716	30.709812
469.164410	23686.828914	30.714829
469.595718	23717.864478	30.719847
469.964372	23752.117986	30.724864
470.767564	23806.140909	30.729882
470.774634	23847.263742	30.734900
471.674169	23878.881285	30.739917
471.891854	23929.008617	30.744935
472.057105	23972.310175	30.749952
472.495070	24014.078049	30.754970
473.238743	24060.504297	30.759988
473.856319	24116.164282	30.765005
474.302530	24148.327284	30.770023
474.742990	24191.605933	30.775040
475.444059	24233.933216	30.780058
476.065474	24271.145383	30.785076
476.559379	24310.924014	30.790093
477.041505	24342.141544	30.795111
477.210940	24384.074610	30.800128
477.766763	24412.476150	30.805146
478.162059	24456.172965	30.810164
478.647859	24501.359392	30.815181
479.170926	24543.865139	30.820199
479.635542	24579.536362	30.825216
480.206256	24626.204089	30.830234
480.758950	24677.770046	30.835252
480.793838	24714.203403	30.840269
481.553764	24755.910347	30.845287
481.573983	24789.599080	30.850304
482.414586	24833.447109	30.855322
482.795467	24877.554262	30.860340
483.173454	24911.641378	30.865357
483.594657	24953.881127	30.870375
483.925322	24993.883912	30.875392
484.419820	25030.399589	30.880410
484.571596	25082.455760	30.885428
485.531530	25132.164137	30.890445
486.119897	25173.408438	30.895463
486.104039	25221.102171	30.900480
486.774199	25255.753532	30.905498
487.218393	25311.837207	30.910516
487.685938	25348.869001	30.915533
487.859643	25398.758721	30.920551
488.369513	25455.223117	30.925568
489.026098	25493.488780	30.930586
489.340478	25552.739481	30.935604
490.380541	25603.221367	30.940621
490.984090	25650.302804	30.945639
491.045569	25700.877516	30.950656
491.735829	25745.285822	30.955674
491.964949	25801.343595	30.960692
492.638875	25851.136078	30.965709
493.252462	25893.746893	30.970727
493.831143	25954.832047	30.975744
494.496844	25996.768935	30.980762
494.964224	26042.407220	30.985780
495.642701	26084.843745	30.990797
496.009113	26120.187440	30.995815
496.386600	26172.689011	31.000832
496.714066	26218.540175	31.005850
497.250334	26267.549124	31.010868
497.631094	26310.934464	31.015885
498.342925	26359.999793	31.020903
498.714125	26417.714186	31.025920
499.403685	26464.193741	31.030938
499.639422	26521.930898	31.035956
500.340701	26570.030165	31.040973
500.834480	26620.040787	31.045991
501.513576	26674.383475	31.051008
502.147806	26710.422199	31.056026
502.608922	26761.905453	31.061044
503.266925	26800.833065	31.066061
504.149228	26846.348035	31.071079
504.216273	26899.546693	31.076096
504.571937	26936.638262	31.081114
505.277279	26987.419332	31.086132
505.577913	27020.643313	31.091149
506.339156	27068.699346	31.096167
506.570624	27125.076470	31.101184
507.294318	27163.754286	31.106202
507.684355	27214.733305	31.111220
508.025656	27268.155846	31.116237
508.720114	27303.431903	31.121255
509.232858	27354.526673	31.126272
509.659263	27398.758918	31.131290
509.926320	27444.607550	31.136308
510.327285	27497.610829	31.141325
510.968813	27547.299993	31.146343
511.371308	27611.918596	31.151360
512.388559	27654.274524	31.156378
512.515296	27715.658342	31.161396
512.952619	27752.807545	31.166413
513.209459	27802.460145	31.171431
513.767774	27862.817212	31.176448
514.447799	27903.989772	31.181466
515.011921	27963.560716	31.186484
515.723554	28010.804199	31.191501
516.134024	28060.955791	31.196519
516.485753	28109.814357	31.201536
517.418803	28152.037163	31.206554
518.117761	28194.005418	31.211572
518.235409	28231.385204	31.216589
518.970179	28274.335155	31.221607
519.465132	28316.252284	31.226624
519.806530	28358.841645	31.231642
520.407742	28405.151737	31.236660
520.766382	28459.404766	31.241677
521.355978	28503.467696	31.246695
521.772475	28554.758584	31.251712
522.070730	28590.834724	31.256730
522.916875	28644.701648	31.261748
523.186745	28687.445612	31.266765
523.938132	28739.514497	31.271783
524.375523	28790.058083	31.276800
524.630798	28835.707261	31.281818
525.251197	28889.318894	31.286836
525.772046	28937.662794	31.291853
526.302423	28990.784859	31.296871
526.629666	29053.402146	31.301888
527.525413	29109.483324	31.306906
528.272118	29161.794014	31.311924
528.622042	29210.867337	31.316941
529.496781	29261.330454	31.321959
529.727674	29321.999137	31.326976
530.423805	29364.491238	31.331994
530.839228	29412.642516	31.337012
530.788540	29467.162006	31.342029
531.785363	29517.280701	31.347047
532.357053	29575.407769	31.352064
532.869878	29625.376547	31.357082
533.750839	29684.219460	31.362100
534.182617	29738.666272	31.367117
534.495694	29785.627146	31.372135
534.738069	29845.563779	31.377152
535.603094	29894.623195	31.382170
536.394014	29956.696886	31.387188
536.674343	30010.210470	31.392205
537.544126	30058.001229	31.397223
537.691955	30114.206224	31.402240
538.395839	30167.741701	31.407258
538.973358	30216.912691	31.412276
539.243659	30264.172189	31.417293
540.162402	30317.704122	31.422311
540.346975	30385.331662	31.427328
541.362616	30419.677449	31.432346
542.322207	30471.865325	31.437364
542.499169	30523.166900	31.442381
543.365584	30565.860907	31.447399
543.796379	30614.953168	31.452416
544.316958	30654.672516	31.457434
544.652212	30706.973860	31.462452
545.029792	30757.116527	31.467469
545.821152	30801.461060	31.472487
546.202709	30857.591891	31.477504
546.695630	30900.957463	31.482522
547.406819	30952.291789	31.487540
547.681895	31018.761442	31.492557
548.416487	31051.937055	31.497575
548.817129	31116.152399	31.502592
549.389145	31156.905596	31.507610
550.167154	31212.224164	31.512628
550.351252	31266.180287	31.517645
550.942100	31314.440265	31.522663
551.449925	31365.351927	31.527680
551.819701	31424.941545	31.532698
552.681501	31476.145195	31.537716
552.762485	31534.852153	31.542733
553.582589	31585.185841	31.547751
553.753439	31640.006698	31.552768
554.381912	31684.443510	31.557786
555.211497	31736.117078	31.562804
555.860923	31791.572328	31.567821
556.169816	31842.218519	31.572839
556.741768	31898.163382	31.577856
557.398446	31954.649751	31.582874
557.525181	32008.418837	31.587892
557.925543	32063.007392	31.592909
558.629676	32118.703891	31.597927
559.211368	32180.242587	31.602944
559.708564	32248.901526	31.607962
560.542284	32310.206490	31.612980
560.968794	32362.500783	31.617997
561.573278	32423.790426	31.623015
561.989784	32481.959058	31.628032
562.398033	32548.636453	31.633050
563.210094	32604.985585	31.638068
563.604178	32684.000695	31.643085
564.749402	32738.909856	31.648103
565.089491	32797.407716	31.653120
565.629161	32855.071237	31.658138
566.294439	32917.002564	31.663156
566.843949	32979.300375	31.668173
567.398604	33026.920955	31.673191
568.029369	33097.274547	31.678208
568.731515	33156.530979	31.683226
569.578494	33200.862856	31.688244
569.591046	33260.454624	31.693261
570.624898	33319.057146	31.698279
571.209334	33372.502171	31.703296
572.115892	33440.612007	31.708314
572.714146	33479.535924	31.713332
572.912145	33541.464689	31.718349
573.519589	33589.851178	31.723367
574.365439	33640.416800	31.728384
574.961935	33699.313835	31.733402
575.584299	33741.443678	31.738420
575.952751	33797.204128	31.743437
576.730087	33858.384904	31.748455
577.360333	33915.008100	31.753472
577.667668	33970.324777	31.758490
578.343256	34020.556736	31.763508
578.547926	34076.714380	31.768525
579.314401	34128.903957	31.773543
579.898368	34189.357319	31.778560
580.758907	34253.432156	31.783578
581.382254	34301.473960	31.788596
581.845065	34366.284037	31.793613
582.401583	34411.642129	31.798631
582.894723	34465.099215	31.803648
583.740768	34524.573064	31.808666
584.251044	34572.735291	31.813684
584.493193	34634.423841	31.818701
585.338931	34687.968422	31.823719
585.476974	34748.671023	31.828736
586.035035	34811.892166	31.833754
586.804271	34858.832010	31.838772
587.071327	34934.204613	31.843789
587.893567	34988.776495	31.848807
588.688848	35045.921934	31.853824
588.995391	35108.721814	31.858842
589.722168	35167.479036	31.863860
590.512948	35231.458452	31.868877
591.119611	35287.859500	31.873895
591.576864	35331.342754	31.878912
592.021617	35396.812826	31.883930
592.885024	35450.877498	31.888948
593.227521	35497.495116	31.893965
594.005513	35543.236017	31.898983
594.266083	35592.095586	31.904000
594.828482	35649.111046	31.909018
595.518018	35704.429791	31.914036
596.187633	35758.382272	31.919053
596.730956	35819.163448	31.924071
597.014864	35873.836553	31.929088
597.673662	35935.056645	31.934106
598.320977	35997.181488	31.939124
598.705982	36064.308195	31.944141
599.475503	36129.490484	31.949159
599.909725	36181.157113	31.954176
600.691541	36247.262539	31.959194
601.365346	36310.277265	31.964212
601.697514	36381.864070	31.969229
602.384861	36441.506228	31.974247
602.925238	36512.872888	31.979264
603.576550	36580.828558	31.984282
604.490422	36642.463338	31.989300
605.022119	36703.924841	31.994317
605.610484	36778.365081	31.999335
606.140227	36832.059849	32.004352
606.891341	36895.714009	32.009370
607.425786	36960.553122	32.014388
608.163309	37027.508293	32.019405
609.099586	37079.744616	32.024423
609.832686	37151.971980	32.029440
610.250496	37217.816074	32.034458
610.975226	37269.573466	32.039476
611.683443	37330.174618	32.044493
612.237211	37390.271260	32.049511
612.940538	37445.315289	32.054528
613.182938	37496.925871	32.059546
613.903981	37555.571867	32.064564
614.421398	37622.379422	32.069581
614.898750	37693.183532	32.074599
615.806735	37747.017280	32.079616
615.814534	37827.289899	32.084634
617.019248	37885.061518	32.089652
617.592009	37963.189588	32.094669
618.024670	38025.148568	32.099687
618.911873	38086.306571	32.104704
619.129183	38155.602521	32.109722
620.028524	38220.486762	32.114740
621.035101	38289.990386	32.119757
621.223248	38350.289572	32.124775
621.896376	38405.493013	32.129792
622.319375	38484.673960	32.134810
623.052131	38536.850290	32.139828
623.645486	38610.081929	32.144845
624.092648	38685.020497	32.149863
625.022963	38744.671049	32.154880
625.346008	38812.862978	32.159898
626.003064	38877.704412	32.164916
626.859936	38951.884993	32.169933
627.271508	39023.087093	32.174951
628.288027	39087.371052	32.179968
628.637246	39154.524546	32.184986
629.385706	39219.800313	32.190004
630.077975	39289.953193	32.195021
630.944687	39344.129933	32.200039
631.558075	39400.994048	32.205056
632.091502	39467.505815	32.210074
632.541622	39523.582894	32.215092
633.078159	39595.322120	32.220109
633.547034	39663.199509	32.225127
634.259833	39718.936993	32.230144
634.747387	39787.998687	32.235162
635.492729	39847.708689	32.240180
636.298413	39909.962734	32.245197
636.625966	39980.974101	32.250215
637.575326	40036.553454	32.255232
637.799572	40099.551478	32.260250
638.458130	40154.027061	32.265268
639.276666	40225.030747	32.270285
639.710738	40294.879772	32.275303
640.327774	40363.091953	32.280320
640.774495	40426.117423	32.285338
641.874366	40500.750218	32.290356
642.621257	40568.657558	32.295373
642.728886	40641.728262	32.300391
643.398099	40711.975616	32.305408
643.975239	40786.503476	32.310426
644.691515	40861.718930	32.315444
645.290997	40934.447392	32.320461
645.557249	41014.252358	32.325479
646.502918	41089.765427	32.330496
647.413104	41164.893208	32.335514
647.859264	41239.536116	32.340532
648.590224	41320.089497	32.345549
648.992579	41397.657372	32.350567
649.892187	41473.612142	32.355584
650.713584	41549.987423	32.360602
651.469988	41623.895471	32.365620
652.384911	41699.741295	32.370637
652.959882	41767.672008	32.375655
654.445220	41834.593630	32.380672
655.022698	41899.859818	32.385690
655.746753	41955.033913	32.390708
656.506342	42016.462892	32.395725
657.017743	42075.779960	32.400743
657.805098	42129.599159	32.405760
658.428730	42201.226751	32.410778
659.203525	42258.543385	32.415796
659.632624	42324.157643	32.420813
659.885486	42379.584598	32.425831
660.802922	42448.490392	32.430848
661.420573	42517.821745	32.435866
661.984614	42591.468690	32.440884
662.636313	42660.817044	32.445901
663.140018	42717.564278	32.450919
664.042046	42781.801120	32.455936
664.405481	42846.774528	32.460954
664.846198	42924.613952	32.465972
665.738348	42990.532826	32.470989
666.038784	43074.688583	32.476007
666.895536	43140.569641	32.481024
667.294735	43223.636239	32.486042
668.089255	43304.977038	32.491060
668.981915	43370.792978	32.496077
669.410654	43454.300902	32.501095
670.018620	43527.783247	32.506112
670.543559	43609.122607	32.511130
670.925956	43680.966288	32.516148
671.784396	43770.289958	32.521165
672.778155	43849.459426	32.526183
673.504640	43930.722635	32.531200
674.254066	44005.916898	32.536218
674.355964	44069.286459	32.541236
675.590494	44154.666043	32.546253
676.515341	44231.714059	32.551271
677.290569	44303.574076	32.556288
677.731960	44374.520233	32.561306
678.552577	44444.125116	32.566324
679.231289	44509.030029	32.571341
679.884994	44576.572714	32.576359
680.355638	44631.894527	32.581376
681.283246	44703.358271	32.586394
681.665748	44766.431154	32.591412
682.567670	44834.034744	32.596429
682.939655	44908.079379	32.601447
683.635656	44972.619906	32.606464
683.898133	45036.619788	32.611482
684.791802	45115.305928	32.616500
685.223694	45196.190743	32.621517
685.946163	45274.814298	32.626535
686.870554	45354.247882	32.631552
687.425371	45436.884860	32.636570
688.091256	45508.622312	32.641588
688.763073	45586.601896	32.646605
689.306313	45673.807911	32.651623
690.019843	45754.304329	32.656640
690.595057	45840.833221	32.661658
691.467197	45930.720647	32.666676
692.252929	46012.421969	32.671693
692.844789	46098.905077	32.676711
693.591736	46178.639895	32.681728
694.513769	46270.049069	32.686746
695.227178	46343.714428	32.691764
696.072750	46427.577092	32.696781
696.105398	46507.908297	32.701799
697.053619	46594.603134	32.706816
697.847712	46684.355465	32.711834
698.500000	46765.864211	32.716852
699.572867	46842.592079	32.721869
700.107703	46929.609465	32.726887
700.774910	47011.609439	32.731904
701.579823	47103.749387	32.736922
701.837818	47190.779025	32.741940
702.615760	47278.594660	32.746957
703.423825	47368.859507	32.751975
704.342100	47458.279142	32.756992
705.100889	47540.591521	32.762010
705.991533	47627.411121	32.767028
706.882329	47705.274754	32.772045
707.408054	47792.351272	32.777063
708.232236	47869.613923	32.782080
708.952059	47952.490352	32.787098
709.491649	48037.645552	32.792116
710.228672	48120.917791	32.797133
710.882379	48199.956438	32.802151
711.777778	48275.936209	32.807168
712.580853	48363.976908	32.812186
713.136054	48450.824156	32.817204
713.987701	48526.834268	32.822221
714.593844	48617.773218	32.827239
715.282857	48693.918275	32.832256
716.103893	48785.949970	32.837274
716.646657	48869.541841	32.842292
717.401741	48943.614604	32.847309
718.064181	49033.191302	32.852327
719.176708	49106.536003	32.857344
719.561873	49203.230835	32.862362
720.442085	49288.351031	32.867380
721.224409	49364.139050	32.872397
721.997330	49447.287931	32.877415
722.562805	49522.149139	32.882432
723.465658	49608.817775	32.887450
724.126209	49696.006962	32.892468
725.198415	49765.586543	32.897485
725.521167	49845.539481	32.902503
726.264606	49916.402624	32.907520
726.800302	49983.987166	32.912538
727.215350	50070.302701	32.917556
728.372274	50146.691952	32.922573
729.192775	50214.312308	32.927591
729.949351	50288.140474	32.932608
730.383594	50361.978021	32.937626
730.892359	50447.944935	32.942644
731.493169	50525.747946	32.947661
732.248149	50608.503660	32.952679
732.584954	50693.640981	32.957696
733.479109	50779.949915	32.962714
734.048463	50867.595356	32.967732
734.883977	50954.034792	32.972749
735.569593	51049.090895	32.977767
736.123970	51146.696092	32.982784
737.307653	51232.257926	32.987802
737.611856	51335.388895	32.992820
738.884605	51422.768871	32.997837
739.584162	51512.922641	33.002855
740.200621	51598.409346	33.007872
741.235232	51688.723301	33.012890
741.886127	51782.083011	33.017908
742.846482	51871.898381	33.022925
743.740801	51961.175460	33.027943
744.490388	52042.655710	33.032960
745.477408	52130.970594	33.037978
745.787171	52215.285118	33.042996
746.661461	52301.907341	33.048013
747.665954	52385.975012	33.053031
748.373447	52467.211288	33.058048
748.819837	52556.394606	33.063066
749.224664	52644.744939	33.068084
750.475117	52735.426057	33.073101
751.159354	52831.236579	33.078119
751.953108	52917.438920	33.083136
752.866061	53005.176126	33.088154
753.455044	53103.676209	33.093172
754.453757	53178.770462	33.098189
755.006149	53270.270820	33.103207
755.853811	53355.309977	33.108224
756.363627	53443.185325	33.113242
757.526726	53541.327280	33.118260
758.283522	53614.871064	33.123277
759.059882	53712.010084	33.128295
759.591549	53795.094250	33.133312
760.598355	53887.969175	33.138330
761.572113	53978.095264	33.143348
762.122038	54069.043743	33.148365
762.928458	54156.582575	33.153383
763.908723	54243.846627	33.158400
764.522919	54325.535670	33.163418
764.934442	54411.182272	33.168436
766.081195	54499.070705	33.173453
766.478978	54604.661238	33.178471
767.370851	54681.977712	33.183488
768.084966	54764.783044	33.188506
768.271467	54866.928450	33.193524
769.608463	54950.421342	33.198541
770.085330	55056.702562	33.203559
770.557962	55149.520135	33.208576
771.845447	55239.669593	33.213594
772.413729	55334.291972	33.218612
773.317995	55425.592472	33.223629
774.172263	55529.317921	33.228647
774.703997	55616.150404	33.233664
775.845805	55698.813071	33.238682
776.713282	55799.062425	33.243700
777.483470	55875.228388	33.248717
778.230936	55963.296786	33.253735
778.399777	56034.817374	33.258752
779.700082	56118.548736	33.263770
780.284437	56208.344981	33.268788
781.360495	56291.267427	33.273805
781.741713	56380.649403	33.278823
782.315891	56466.233734	33.283840
782.873336	56552.800651	33.288858
783.681684	56658.511119	33.293876
784.756840	56746.844731	33.298893
785.129804	56848.343873	33.303911
785.528830	56937.219863	33.308928
786.436773	57038.460864	33.313946
787.291017	57142.896146	33.318964
788.236490	57241.572683	33.323981
789.016422	57350.931401	33.328999
789.474478	57455.743490	33.334016
790.787945	57559.763745	33.339034
791.337166	57663.329566	33.344052
791.890058	57765.024767	33.349069
792.800562	57875.192587	33.354087
793.519556	57974.441025	33.359104
794.607238	58089.124420	33.364122
794.857032	58190.372663	33.369140
796.259297	58311.792492	33.374157
797.234891	58418.318759	33.379175
797.907215	58527.531048	33.384192
798.902955	58619.747355	33.389210
799.610742	58729.365650	33.394228
800.524509	58828.484964	33.399245
801.359853	58948.845888	33.404263
802.256168	59045.877307	33.409280
803.501536	59134.237508	33.414298
804.184520	59251.155838	33.419316
804.640603	59337.941111	33.424333
805.895786	59436.640383	33.429351
806.457882	59540.750909	33.434368
807.312082	59645.022215	33.439386
807.732665	59745.674877	33.444404
808.695730	59855.016885	33.449421
809.711945	59953.606520	33.454439
810.446056	60054.853507	33.459456
811.501862	60152.976192	33.464474
812.073250	60268.383042	33.469492
813.471125	60359.156639	33.474509
814.298898	60456.774968	33.479527
814.652522	60564.521445	33.484544
815.317748	60658.704109	33.489562
816.328643	60757.639819	33.494580
817.449071	60853.827489	33.499597
818.164450	60961.377180	33.504615
818.887595	61063.743389	33.509632
819.921655	61167.234295	33.514650
820.750072	61270.424751	33.519668
821.205593	61354.450333	33.524685
822.758301	61459.127362	33.529703
823.459805	61556.942493	33.534720
824.379310	61649.747703	33.539738
824.769687	61754.378304	33.544756
825.689202	61843.973499	33.549773
826.513972	61939.102738	33.554791
827.341721	62042.398326	33.559808
828.296265	62130.269735	33.564826
828.847326	62228.454273	33.569844
829.506823	62340.394442	33.574861
830.626014	62425.926459	33.579879
831.239745	62532.230713	33.584896
832.098033	62622.496804	33.589914
833.038031	62716.814149	33.594932
833.664879	62808.472019	33.599949
834.492319	62884.863495	33.604967
835.175625	62984.666906	33.609984
836.410128	63079.057300	33.615002
836.628514	63174.678128	33.620020
837.712704	63267.842670	33.625037
838.611988	63363.983871	33.630055
839.249359	63473.740413	33.635072
839.901247	63555.732372	33.640090
840.700321	63677.960285	33.645108
841.219379	63775.455818	33.650125
842.230531	63889.659814	33.655143
842.537058	63993.316873	33.660160
843.972559	64104.651515	33.665178
844.788485	64227.689018	33.670196
845.256738	64327.186791	33.675213
846.380813	64446.558760	33.680231
846.915070	64564.770983	33.685248
847.987168	64668.424898	33.690266
848.715748	64793.895027	33.695284
850.034434	64907.604924	33.700301
850.867219	65026.965182	33.705319
851.411058	65144.401545	33.710336
852.505460	65247.517309	33.715354
853.280666	65382.990558	33.720372
854.094089	65486.874657	33.725389
855.184568	65609.198476	33.730407
855.916439	65716.340302	33.735424
857.076470	65827.634890	33.740442
857.996623	65944.710057	33.745460
858.954596	66051.898390	33.750477
860.195304	66165.729185	33.755495
860.914741	66272.091981	33.760512
862.217428	66374.982872	33.765530
863.017230	66481.289183	33.770548
863.680757	66577.003722	33.775565
864.501219	66690.843647	33.780583
864.990708	66797.411507	33.785600
866.123773	66903.057902	33.790618
866.751871	67025.681405	33.795636
867.762144	67129.920416	33.800653
868.979395	67235.276374	33.805671
869.440583	67353.219258	33.810688
870.404389	67463.549709	33.815706
870.845647	67579.688949	33.820724
871.851339	67699.332957	33.825741
872.991150	67822.432832	33.830759
873.532031	67929.314029	33.835776
874.381847	68032.053977	33.840794
875.439357	68155.852238	33.845812
876.392172	68268.534386	33.850829
877.218857	68385.967345	33.855847
877.991058	68511.427145	33.860864
879.037555	68611.355383	33.865882
879.697810	68729.867339	33.870900
880.722871	68864.297345	33.875917
881.842484	68964.588197	33.880935
882.947943	69094.599346	33.885952
883.800165	69195.536180	33.890970
884.904109	69310.696404	33.895988
885.500775	69416.962527	33.901005
886.576808	69521.316229	33.906023
886.883012	69628.826489	33.911040
887.977713	69735.479735	33.916058
889.150496	69856.138904	33.921076
889.830573	69972.605800	33.926093
891.081492	70071.337294	33.931111
891.510190	70165.526062	33.936128
892.392633	70264.313061	33.941146
893.196811	70370.808853	33.946164
894.052408	70486.857473	33.951181
894.928076	70574.910089	33.956199
895.824324	70702.556429	33.961216
896.873663	70792.503513	33.966234
897.169558	70907.565670	33.971252
898.063162	71016.130272	33.976269
899.317942	71137.194108	33.981287
899.696260	71254.154174	33.986304
900.953386	71360.934077	33.991322
901.692407	71488.389751	33.996340
902.604982	71594.728229	34.001357
903.675781	71715.939566	34.006375
904.345378	71841.486416	34.011392
905.447662	71959.785020	34.016410
906.709537	72076.287228	34.021428
907.459221	72189.156383	34.026445
908.683434	72307.221713	34.031463
909.220315	72427.747503	34.036480
910.687730	72536.990036	34.041498
911.380630	72654.639212	34.046516
911.900550	72779.533262	34.051533
913.114218	72891.722239	34.056551
913.773800	73012.205681	34.061568
914.543418	73134.726910	34.066586
915.675115	73255.513066	34.071604
916.640120	73381.721938	34.076621
917.440302	73509.071852	34.081639
918.630758	73635.953218	34.086656
919.474621	73757.561305	34.091674
920.227088	73871.526491	34.096692
921.212462	73992.916433	34.101709
922.217693	74118.174261	34.106727
923.203016	74244.878055	34.111744
924.219345	74370.514953	34.116762
925.302548	74489.209915	34.121780
926.128536	74604.735219	34.126797
927.425780	74729.214607	34.131815
927.972151	74853.363505	34.136832
928.940144	74973.718197	34.141850
930.056321	75098.197994	34.146868
930.661812	75215.204982	34.151885
932.017726	75341.613478	34.156903
932.551353	75469.448926	34.161920
933.633289	75582.046629	34.166938
934.466144	75708.663897	34.171956
935.687568	75832.643426	34.176973
936.686914	75952.195018	34.181991
937.344947	76072.859957	34.187008
938.387106	76189.116800	34.192026
939.266055	76318.645730	34.197044
940.144383	76440.857486	34.202061
941.061545	76556.966153	34.207079
942.216180	76691.208098	34.212096
943.043401	76810.622006	34.217114
943.971124	76928.894058	34.222132
944.801003	77059.143837	34.227149
945.709035	77193.303089	34.232167
946.647147	77317.850109	34.237184
947.834136	77438.447639	34.242202
948.613424	77565.685254	34.247220
949.537684	77695.676454	34.252237
950.712592	77823.457350	34.257255
951.129768	77957.443022	34.262272
952.361543	78066.340807	34.267290
953.425188	78191.131280	34.272308
954.122155	78319.455804	34.277325
955.089367	78415.241919	34.282343
955.936125	78536.464606	34.287360
956.670353	78655.707657	34.292378
957.897235	78773.048081	34.297396
958.437085	78904.925327	34.302413
960.148570	79021.750440	34.307431
960.721548	79157.064885	34.312448
961.387177	79263.734214	34.317466
962.386982	79399.219910	34.322484
962.946334	79532.318488	34.327501
963.987549	79660.062353	34.332519
964.980227	79790.560429	34.337536
966.015056	79927.922312	34.342554
967.148512	80063.554366	34.347572
967.808238	80204.414986	34.352589
969.002444	80344.346727	34.357607
969.541580	80475.284334	34.362624
970.813202	80625.491315	34.367642
971.672819	80761.400566	34.372660
972.525858	80906.642950	34.377677
973.826907	81038.710410	34.382695
974.667275	81182.299158	34.387712
975.683736	81335.229058	34.392730
976.767098	81472.617558	34.397748
977.513893	81622.184032	34.402765
978.522593	81760.010479	34.407783
979.674184	81920.646607	34.412800
980.724220	82067.230331	34.417818
981.749838	82205.062986	34.422836
982.780925	82350.677357	34.427853
984.074154	82492.636758	34.432871
984.610101	82644.870350	34.437888
985.655978	82782.152692	34.442906
986.800268	82922.545028	34.447924
987.338642	83079.545187	34.452941
988.919531	83218.026013	34.457959
989.659425	83365.941007	34.462976
990.803375	83517.491419	34.467994
992.190798	83651.951246	34.473012
992.649994	83801.060630	34.478029
994.047340	83944.675773	34.483047
994.965772	84096.767111	34.488064
996.665796	84240.954102	34.493082
997.360884	84373.159907	34.498100
998.246612	84513.737530	34.503117
999.487328	84649.796566	34.508135
1000.537466	84796.353310	34.513152
1001.257621	84942.231567	34.518170
1002.636416	85066.140642	34.523188
1003.343600	85219.565043	34.528205
1004.175694	85347.039776	34.533223
1004.818309	85508.303841	34.538240
1005.987175	85653.428972	34.543258
1007.423372	85793.682841	34.548276
1008.302013	85941.635565	34.553293
1009.138143	86084.635352	34.558311
1010.159301	86227.111853	34.563328
1010.907665	86379.619524	34.568346
1012.117959	86522.104508	34.573364
1012.957343	86670.485948	34.578381
1013.883117	86814.038526	34.583399
1015.355003	86964.804091	34.588416
1016.373026	87123.093670	34.593434
1017.286470	87260.791319	34.598452
1018.413001	87405.889974	34.603469
1019.149238	87538.214402	34.608487
1020.329747	87677.268821	34.613504
1021.085044	87819.191404	34.618522
1021.913637	87947.946434	34.623540
1022.794392	88091.140847	34.628557
1024.289739	88230.418567	34.633575
1025.220561	88369.239885	34.638592
1026.172864	88500.255638	34.643610
1027.466352	88635.955639	34.648628
1028.180822	88788.883126	34.653645
1029.352171	88928.028651	34.658663
1030.193076	89071.925353	34.663680
1031.055415	89211.699517	34.668698
1032.206776	89357.154046	34.673716
1032.886729	89511.825890	34.678733
1034.355593	89654.356548	34.683751
1035.678337	89805.658433	34.688768
1036.282525	89956.301653	34.693786
1037.349892	90097.622933	34.698804
1038.434970	90259.820779	34.703821
1039.410357	90406.658802	34.708839
1040.429889	90566.686109	34.713856
1041.355383	90711.243187	34.718874
1042.521407	90869.533149	34.723892
1043.570535	91026.027057	34.728909
1044.718124	91187.619555	34.733927
1045.930784	91341.702422	34.738944
1046.945316	91495.319030	34.743962
1048.237452	91639.194453	34.748980
1048.791364	91804.819631	34.753997
1050.286254	91960.347126	34.759015
1051.234037	92113.067271	34.764032
1052.239908	92272.392902	34.769050
1053.314120	92425.518167	34.774068
1053.928813	92593.929908	34.779085
1055.503494	92742.683085	34.784103
1056.681084	92898.471578	34.789120
1057.528019	93062.702345	34.794138
1059.089509	93213.023959	34.799156
1059.930675	93388.264966	34.804173
1060.901374	93528.204377	34.809191
1062.172639	93698.097566	34.814208
1063.129372	93853.757748	34.819226
1063.905969	94001.492188	34.824244
1064.953223	94163.222261	34.829261
1066.177257	94331.962954	34.834279
1067.227846	94485.851915	34.839296
1068.270684	94666.436421	34.844314
1069.850032	94817.897954	34.849332
1070.946985	94973.143229	34.854349
1071.798826	95134.323279	34.859367
1072.956524	95293.054703	34.864384
1073.834871	95448.870828	34.869402
1075.541083	95591.897049	34.874420
1076.055688	95749.933789	34.879437
1077.489963	95902.761610	34.884455
1078.578858	96065.320151	34.889472
1079.805863	96215.348191	34.894490
1080.759476	96377.513332	34.899508
1081.473165	96531.704899	34.904525
1082.677575	96686.442997	34.909543
1083.976058	96846.059962	34.914560
1084.667556	96998.795733	34.919578
1086.053408	97159.324505	34.924596
1087.151974	97327.327603	34.929613
1087.743511	97477.310005	34.934631
1089.420598	97633.045672	34.939648
1090.127498	97799.274448	34.944666
1091.573863	97942.097516	34.949684
1092.480640	98097.982408	34.954701
1093.303077	98236.345791	34.959719
1094.552988	98387.997392	34.964736
1095.457841	98542.809097	34.969754
1096.856038	98681.649507	34.974772
1097.820450	98828.583749	34.979789
1098.596783	98971.694347	34.984807
1099.792420	99126.353912	34.989824
1100.695295	99288.710785	34.994842
1101.753525	99441.109457	34.999860
1102.638476	99604.693216	35.004877
1103.796533	99764.364500	35.009895
1105.222047	99924.030553	35.014912
1105.967711	100100.252377	35.019930
1107.106606	100256.618637	35.024948
1107.798501	100428.362692	35.029965
1108.847453	100596.984457	35.034983
1110.350665	100774.852142	35.040000
1111.242336	100941.590072	35.045018
1112.471467	101115.871147	35.050036
1113.510545	101294.281363	35.055053
1114.489160	101475.134157	35.060071
1115.648658	101649.873570	35.065088
1116.695585	101835.706958	35.070106
1117.898057	102002.564988	35.075124
1119.064448	102182.486243	35.080141
1120.464805	102360.641472	35.085159
1121.898113	102538.140292	35.090176
1122.677532	102720.237773	35.095194
1123.794908	102898.392818	35.100212
1125.110150	103070.994843	35.105229
1126.287448	103246.045998	35.110247
1127.227942	103426.937690	35.115264
1128.384789	103607.490922	35.120282
1130.003362	103789.678759	35.125300
1130.931443	103979.530053	35.130317
1131.662283	104160.018211	35.135335
1132.905381	104332.355533	35.140352
1134.172870	104530.184090	35.145370
1135.335651	104701.346620	35.150388
1136.614681	104890.880512	35.155405
1137.819755	105073.120277	35.160423
1139.112792	105242.668994	35.165440
1140.058154	105438.809835	35.170458
1141.460753	105609.039372	35.175476
1142.216499	105801.212016	35.180493
1143.615578	105982.792700	35.185511
1145.023889	106156.191166	35.190528
1145.807797	106338.749903	35.195546
1147.323496	106521.556216	35.200564
1148.329767	106701.268888	35.205581
1149.439389	106872.783529	35.210599
1150.873687	107055.264977	35.215616
1151.923877	107241.357661	35.220634
1153.213440	107417.076502	35.225652
1154.281738	107602.598723	35.230669
1155.232487	107782.530486	35.235687
1156.494574	107962.513314	35.240704
1157.561464	108142.048288	35.245722
1158.908865	108323.590067	35.250740
1159.927166	108497.169490	35.255757
1160.842155	108687.702512	35.260775
1162.250984	108862.486392	35.265792
1163.431436	109059.362215	35.270810
1164.574159	109232.127765	35.275828
1165.548411	109411.952484	35.280845
1166.351293	109597.076254	35.285863
1167.515990	109786.891681	35.290880
1168.781449	109956.538067	35.295898
1169.828392	110140.231772	35.300916
1171.125072	110313.878115	35.305933
1172.219477	110485.519522	35.310951
1173.319865	110663.659515	35.315968
1174.805439	110836.707903	35.320986
1175.781837	111016.720172	35.326004
1176.965391	111191.860241	35.331021
1177.897398	111380.078347	35.336039
1179.041564	111555.607279	35.341056
1180.126589	111749.465229	35.346074
1181.207311	111927.794005	35.351092
1182.383777	112115.064595	35.356109
1183.746012	112306.296285	35.361127
1185.238124	112488.842584	35.366144
1186.064150	112682.230467	35.371162
1187.478191	112860.484800	35.376180
1188.943871	113059.825180	35.381197
1189.519978	113252.726248	35.386215
1190.919759	113450.585391	35.391232
1192.371589	113644.598622	35.396250
1193.672962	113829.313620	35.401268
1194.774567	114021.765715	35.406285
1196.113682	114222.554248	35.411303
1197.407302	114409.339434	35.416320
1198.676004	114594.749011	35.421338
1199.799657	114796.856870	35.426356
1201.209846	114987.009377	35.431373
1202.353746	115181.780942	35.436391
1203.560962	115363.189435	35.441408
1204.989183	115557.625179	35.446426
1205.945788	115760.134955	35.451444
1207.244900	115949.336694	35.456461
1208.329694	116143.579817	35.461479
1209.679799	116330.634410	35.466496
1210.912268	116535.688819	35.471514
1211.964472	116725.329300	35.476532
1213.468197	116926.071751	35.481549
1214.279205	117122.888208	35.486567
1215.514473	117313.630000	35.491584
1216.658996	117523.343466	35.496602
1217.576655	117724.885267	35.501620
1219.093300	117928.888988	35.506637
1220.277732	118141.527333	35.511655
1221.432039	118347.405857	35.516672
1222.830574	118556.730049	35.521690
1224.162997	118756.183088	35.526708
1225.007940	118957.187954	35.531725
1226.305025	119170.537489	35.536743
1227.526137	119377.654075	35.541760
1228.806926	119594.101260	35.546778
1230.121432	119801.927700	35.551796
1231.411608	120008.365739	35.556813
1232.837282	120218.521046	35.561831
1234.185119	120413.889837	35.566848
1235.309994	120619.624523	35.571866
1236.805494	120837.122517	35.576884
1238.196860	121023.275492	35.581901
1239.446698	121226.776115	35.586919
1240.830951	121424.426606	35.591936
1241.542317	121630.781602	35.596954
1242.943441	121828.026476	35.601972
1244.364671	122023.773960	35.606989
1245.340516	122223.740346	35.612007
1246.790667	122430.498358	35.617024
1248.131972	122632.878286	35.622042
1249.220813	122833.831244	35.627060
1250.653783	123024.945033	35.632077
1251.824594	123218.764743	35.637095
1252.822865	123398.458189	35.642112
1254.062431	123589.163976	35.647130
1255.535431	123773.571718	35.652148
1256.775188	123957.106650	35.657165
1257.530046	124154.258227	35.662183
1258.766304	124343.803364	35.667200
1260.024492	124543.117515	35.672218
1261.656969	124742.662609	35.677236
1263.037854	124933.784433	35.682253
1263.947730	125144.794753	35.687271
1265.192058	125339.642503	35.692288
1266.322210	125537.501471	35.697306
1267.368029	125737.137379	35.702324
1268.583184	125939.319486	35.707341
1269.773381	126150.341114	35.712359
1270.918012	126357.315886	35.717376
1272.205516	126570.833869	35.722394
1273.557447	126798.614363	35.727412
1275.080981	127001.880535	35.732429
1276.024094	127229.478286	35.737447
1277.364133	127439.140439	35.742464
1278.864014	127669.818133	35.747482
1279.678412	127884.906368	35.752500
1281.146552	128102.549828	35.757517
1282.476335	128332.043730	35.762535
1283.809375	128549.826721	35.767552
1285.036454	128778.542330	35.772570
1286.558178	129006.602481	35.777588
1287.930648	129216.169819	35.782605
1289.145797	129457.022953	35.787623
1290.451291	129672.638062	35.792640
1291.886027	129899.312047	35.797658
1292.642459	130133.413837	35.802676
1294.448707	130360.232538	35.807693
1295.661428	130589.001689	35.812711
1297.332984	130812.119079	35.817728
1298.521021	131039.957508	35.822746
1300.159904	131267.786432	35.827764
1301.464203	131490.386155	35.832781
1302.365478	131712.508942	35.837799
1303.743564	131934.782642	35.842816
1305.246192	132175.938453	35.847834
1306.560744	132386.892692	35.852852
1307.928732	132613.546289	35.857869
1309.158814	132844.293620	35.862887
1310.385995	133063.202584	35.867904
1312.024041	133294.988615	35.872922
1313.011045	133519.886000	35.877940
1314.532872	133746.915099	35.882957
1315.847837	133978.746726	35.887975
1317.477391	134208.486906	35.892992
1319.026248	134422.483639	35.898010
1319.965456	134651.656433	35.903028
1321.491493	134874.306149	35.908045
1323.015176	135091.354099	35.913063
1324.670900	135314.923533	35.918080
1325.858431	135535.541788	35.923098
1326.884907	135751.015418	35.928116
1328.550320	135958.220022	35.933133
1329.755155	136187.841359	35.938151
1331.004664	136400.252210	35.943168
1332.149967	136624.371265	35.948186
1333.488000	136842.868692	35.953204
1334.923209	137064.305630	35.958221
1336.226677	137294.463469	35.963239
1337.287639	137504.135840	35.968256
1338.908373	137721.768149	35.973274
1339.977724	137939.416921	35.978292
1341.320283	138140.703902	35.983309
1342.557770	138346.637357	35.988327
1344.007857	138558.356721	35.993344
1345.286509	138759.074697	35.998362
1346.530030	138980.314996	36.003380
1347.625505	139189.180630	36.008397
1348.912409	139411.557718	36.013415
1350.127096	139619.708907	36.018432
1351.438660	139839.815045	36.023450
1352.385189	140073.246043	36.028468
1353.886254	140298.066066	36.033485
1355.505220	140530.412681	36.038503
1356.651073	140764.893231	36.043520
1358.076188	140993.635815	36.048538
1359.259564	141230.332352	36.053556
1360.774330	141452.963944	36.058573
1361.824198	141697.560231	36.063591
1363.212252	141936.586315	36.068608
1364.804831	142173.842990	36.073626
1366.045192	142414.443789	36.078644
1368.049791	142654.083005	36.083661
1369.135618	142891.149311	36.088679
1370.860138	143128.973967	36.093696
1372.534117	143366.821262	36.098714
1373.352019	143599.536288	36.103732
1374.613327	143843.110770	36.108749
1376.323241	144077.672469	36.113767
1377.705521	144320.342542	36.118784
1379.358354	144566.342827	36.123802
1380.307050	144819.588214	36.128820
1382.012298	145046.028175	36.133837
1383.437553	145282.572448	36.138855
1384.709554	145531.140599	36.143872
1386.230133	145769.435093	36.148890
1387.419246	146017.183289	36.153908
1389.156777	146258.869295	36.158925
1390.288191	146515.812256	36.163943
1392.240122	146753.103462	36.168960
1393.325425	146988.142475	36.173978
1394.540191	147243.364683	36.178996
1396.122942	147477.246631	36.184013
1397.488568	147726.638696	36.189031
1398.825171	147969.556410	36.194048
1400.600271	148217.577823	36.199066
1401.498045	148462.422987	36.204084
1403.283495	148706.983565	36.209101
1404.466107	148961.855196	36.214119
1406.242463	149205.076163	36.219136
1407.853965	149450.875281	36.224154
1409.161922	149696.015918	36.229172
1410.472462	149936.274653	36.234189
1411.809583	150188.934916	36.239207
1413.214566	150433.125767	36.244224
1414.741643	150668.495621	36.249242
1415.927310	150914.615688	36.254260
1417.311179	151162.201285	36.259277
1418.613874	151410.613678	36.264295
1419.688271	151663.504790	36.269312
1421.310940	151914.962474	36.274330
1422.704052	152175.807917	36.279348
1424.022416	152424.680952	36.284365
1425.756197	152687.985050	36.289383
1427.062559	152935.683744	36.294400
1428.840055	153192.071106	36.299418
1429.979795	153451.102459	36.304436
1431.392348	153694.691376	36.309453
1432.887359	153950.534264	36.314471
1434.097075	154185.356618	36.319488
1435.652805	154422.939236	36.324506
1436.476233	154657.155964	36.329524
1438.156765	154908.712347	36.334541
1439.444805	155154.867942	36.339559
1440.682449	155394.652780	36.344576
1442.231630	155645.753543	36.349594
1443.762231	155896.833599	36.354612
1444.993481	156141.571284	36.359629
1446.440198	156402.245852	36.364647
1447.698054	156651.980346	36.369664
1449.500218	156908.476687	36.374682
1450.512221	157177.372310	36.379700
1452.027646	157437.014722	36.384717
1453.411456	157703.442122	36.389735
1454.649272	157961.332391	36.394752
1456.187033	158240.081313	36.399770
1457.587314	158511.281253	36.404788
1458.949252	158790.760740	36.409805
1460.433940	159070.526326	36.414823
1461.407053	159348.982857	36.419840
1463.030618	159626.344248	36.424858
1464.813892	159927.075115	36.429876
1465.885449	160209.111487	36.434893
1467.839407	160499.833930	36.439911
1469.066290	160786.453841	36.444928
1471.022271	161067.385696	36.449946
1472.218377	161368.718813	36.454964
1474.404481	161630.395633	36.459981
1475.567582	161931.953926	36.464999
1477.215949	162219.820768	36.470016
1478.914874	162487.191174	36.475034
1480.571981	162784.081100	36.480052
1481.973498	163054.308139	36.485069
1483.657528	163333.739453	36.490087
1485.090963	163620.281029	36.495104
1486.729148	163892.428155	36.500122
1488.059954	164171.974044	36.505140
1489.889021	164453.837426	36.510157
1491.336426	164734.217773	36.515175
1492.733528	165017.653380	36.520192
1494.204011	165286.373133	36.525210
1495.942913	165575.338672	36.530228
1497.326205	165846.702738	36.535245
1498.842651	166138.576302	36.540263
1500.258272	166425.621458	36.545280
1502.008243	166696.866725	36.550298
1503.827339	166990.446924	36.555316
1504.974999	167253.116078	36.560333
1506.491435	167537.284105	36.565351
1507.481515	167822.276862	36.570368
1509.171681	168107.333395	36.575386
1510.479505	168406.603186	36.580404
1512.001754	168696.538399	36.585421
1513.733241	168986.758122	36.590439
1514.917711	169277.374624	36.595456
1516.753449	169567.898054	36.600474
1518.270608	169868.424494	36.605492
1519.905705	170157.068700	36.610509
1521.122439	170441.837371	36.615527
1522.344897	170741.035022	36.620544
1524.306977	171026.407444	36.625562
1525.639752	171336.199342	36.630580
1527.136717	171617.857967	36.635597
1528.564706	171915.036866	36.640615
1530.104933	172211.577282	36.645632
1531.597127	172506.566607	36.650650
1533.198813	172796.019421	36.655668
1534.467911	173079.361454	36.660685
1536.216562	173359.694454	36.665703
1537.563696	173645.019339	36.670720
1539.130624	173910.905767	36.675738
1540.536816	174200.500901	36.680756
1541.925269	174482.651265	36.685773
1543.636000	174774.483838	36.690791
1545.161728	175062.554167	36.695808
1547.097077	175346.510115	36.700826
1547.918265	175645.817525	36.705844
1549.484391	175933.797462	36.710861
1550.907641	176236.993981	36.715879
1552.344495	176541.751127	36.720896
1553.923579	176837.057008	36.725914
1555.173225	177150.161604	36.730932
1556.952120	177466.213971	36.735949
1558.641443	177771.013043	36.740967
1560.221324	178078.890714	36.745984
1561.958599	178389.396814	36.751002
1563.146229	178709.082923	36.756020
1564.533475	179037.914255	36.761037
1566.314870	179345.537827	36.766055
1567.743034	179670.101956	36.771072
1569.352694	179981.108379	36.776090
1571.116410	180322.615851	36.781108
1572.510390	180642.812912	36.786125
1574.072570	180965.674912	36.791143
1575.522163	181298.013330	36.796160
1577.658615	181629.643813	36.801178
1578.733723	181965.691034	36.806196
1580.492986	182302.338129	36.811213
1582.398332	182623.719257	36.816231
1583.765602	182956.373553	36.821248
1585.788228	183302.261832	36.826266
1587.452853	183644.263956	36.831284
1589.265282	183973.677709	36.836301
1590.766975	184303.474804	36.841319
1592.055572	184640.391879	36.846336
1593.966784	184971.445406	36.851354
1595.581172	185297.244136	36.856372
1596.830559	185637.232836	36.861389
1598.737504	185955.244092	36.866407
1600.433523	186295.213765	36.871424
1601.932415	186625.748602	36.876442
1603.779920	186965.506869	36.881460
1605.435327	187295.461217	36.886477
1607.227014	187624.468300	36.891495
1608.703366	187959.889018	36.896512
1610.176489	188279.495492	36.901530
1611.784241	188617.538658	36.906548
1613.003493	188952.639454	36.911565
1615.005242	189287.777914	36.916583
1616.525328	189640.325559	36.921600
1618.393589	189977.990764	36.926618
1619.694797	190311.016541	36.931636
1621.149519	190646.748128	36.936653
1622.948023	190982.323238	36.941671
1624.621831	191333.268642	36.946688
1626.281645	191663.297488	36.951706
1627.885724	192009.497790	36.956724
1629.248281	192350.852425	36.961741
1630.960889	192689.726388	36.966759
1632.522557	193038.872004	36.971776
1634.394192	193381.570053	36.976794
1635.897010	193728.520302	36.981812
1637.224133	194070.829650	36.986829
1639.103822	194409.939220	36.991847
1640.578636	194755.147771	36.996864
1642.367325	195077.467287	37.001882
1644.012919	195406.299445	37.006900
1645.763474	195729.656854	37.011917
1646.906366	196055.045989	37.016935
1648.511327	196386.924069	37.021952
1650.299067	196712.641593	37.026970
1651.721659	197051.789715	37.031988
1653.068572	197387.295663	37.037005
1655.173504	197718.970866	37.042023
1656.528375	198068.101633	37.047040
1658.119099	198412.281871	37.052058
1660.103774	198748.489096	37.057076
1661.251603	199101.404730	37.062093
1663.058440	199451.267782	37.067111
1664.861629	199806.732279	37.072128
1666.330188	200159.689206	37.077146
1668.014291	200529.866763	37.082164
1669.726932	200886.380115	37.087181
1671.395030	201238.827023	37.092199
1672.667837	201599.352544	37.097216
1674.327170	201963.802787	37.102234
1676.388110	202334.740054	37.107252
1677.658499	202712.462943	37.112269
1679.861491	203077.209867	37.117287
1680.936734	203454.054631	37.122304
1682.521127	203826.220883	37.127322
1684.426997	204205.903343	37.132340
1686.506131	204592.021946	37.137357
1687.960935	204976.163308	37.142375
1689.400239	205370.225735	37.147392
1691.112469	205751.496972	37.152410
1692.941073	206134.096788	37.157428
1694.830190	206522.199183	37.162445
1696.539139	206914.790089	37.167463
1697.675986	207309.166225	37.172480
1699.547536	207711.524047	37.177498
1701.589477	208097.120152	37.182516
1703.074532	208497.310940	37.187533
1705.003873	208883.615054	37.192551
1706.620574	209296.384247	37.197568
1708.022049	209691.375809	37.202586
1709.970570	210087.104244	37.207604
1711.714363	210500.036153	37.212621
1713.449567	210898.800363	37.217639
1715.368226	211308.558158	37.222656
1716.799346	211710.500111	37.227674
1718.731482	212113.656383	37.232692
1720.643054	212517.529008	37.237709
1722.514934	212918.235419	37.242727
1724.099606	213340.045156	37.247744
1725.579702	213735.257981	37.252762
1727.928233	214137.440285	37.257780
1729.467175	214541.739065	37.262797
1731.216395	214940.163464	37.267815
1732.798317	215354.719224	37.272832
1735.074859	215753.771093	37.277850
1736.740109	216156.862252	37.282868
1738.403914	216565.720646	37.287885
1740.142182	216949.856247	37.292903
1741.761674	217354.179021	37.297920
1743.266379	217764.897341	37.302938
1745.275920	218175.483158	37.307956
1746.905355	218581.002956	37.312973
1748.668086	218977.028716	37.317991
1750.236002	219385.889046	37.323008
1751.787828	219789.394517	37.328026
1753.660066	220207.605285	37.333044
1755.320655	220607.489279	37.338061
1757.508792	220990.194130	37.343079
1758.945126	221387.527351	37.348096
1760.608967	221771.286695	37.353114
1762.402058	222152.587690	37.358132
1763.864706	222551.952661	37.363149
1765.757502	222981.041473	37.368167
1767.572054	223410.830595	37.373184
1769.008141	223800.552482	37.378202
1771.235757	224205.587915	37.383220
1772.688745	224604.123336	37.388237
1774.710943	224992.329930	37.393255
1776.627369	225396.201573	37.398272
1778.209423	225808.968962	37.403290
1779.837572	226210.528668	37.408308
1781.353142	226616.832671	37.413325
1783.081222	227029.833925	37.418343
1785.055645	227442.567202	37.423360
1786.919368	227863.498985	37.428378
1788.956669	228280.110748	37.433396
1790.051448	228695.711040	37.438413
1792.283330	229125.069729	37.443431
1793.983524	229544.585882	37.448448
1795.495619	229971.195766	37.453466
1797.562236	230401.423860	37.458484
1799.236718	230830.143134	37.463501
1801.087641	231255.989599	37.468519
1803.044950	231694.952059	37.473536
1804.598860	232136.217711	37.478554
1806.764208	232572.328789	37.483572
1808.558521	233007.689513	37.488589
1810.218538	233440.736674	37.493607
1812.452956	233891.699730	37.498624
1814.128365	234327.921862	37.503642
1816.230335	234759.781804	37.508660
1818.073820	235197.680305	37.513677
1819.770758	235629.101269	37.518695
1821.832102	236077.939494	37.523712
1823.463416	236519.737339	37.528730
1825.532279	236952.624118	37.533748
1827.380931	237395.023173	37.538765
1829.397865	237829.978067	37.543783
1831.183964	238275.640897	37.548800
1833.117078	238707.715711	37.553818
1835.242585	239140.851946	37.558836
1836.740668	239583.212080	37.563853
1838.511733	240020.244368	37.568871
1840.791995	240458.463538	37.573888
1842.479488	240900.541001	37.578906
1844.455470	241330.683338	37.583924
1846.150772	241778.832333	37.588941
1848.387414	242215.131395	37.593959
1849.980942	242659.132782	37.598976
1852.063684	243090.378255	37.603994
1854.263861	243519.598228	37.609012
1855.545529	243959.639681	37.614029
1857.460790	244391.422920	37.619047
1859.492531	244831.748286	37.624064
1861.535771	245268.414402	37.629082
1863.252554	245702.493157	37.634100
1864.641620	246149.759889	37.639117
1866.506094	246585.314197	37.644135
1868.269632	247028.633612	37.649152
1870.081854	247486.526821	37.654170
1872.319182	247920.979664	37.659188
1874.477310	248365.708882	37.664205
1875.977067	248813.976724	37.669223
1878.141284	249255.860757	37.674240
1880.177664	249689.281719	37.679258
1882.276424	250099.347344	37.684276
1883.633994	250519.239703	37.689293
1885.633286	250921.955528	37.694311
1887.402303	251342.568093	37.699328
1888.848829	251769.508807	37.704346
1890.783985	252186.766723	37.709364
1892.687639	252623.057106	37.714381
1894.132633	253047.077543	37.719399
1896.134495	253474.537306	37.724416
1897.991413	253917.085351	37.729434
1900.376920	254343.389855	37.734452
1901.826273	254787.326584	37.739469
1903.466923	255222.874223	37.744487
1905.549540	255664.776058	37.749504
1907.181126	256115.415031	37.754522
1909.185044	256564.824084	37.759540
1910.937357	257030.329666	37.764557
1912.805978	257483.216080	37.769575
1914.721425	257950.854131	37.774592
1916.256409	258405.040478	37.779610
1918.433866	258869.205847	37.784628
1920.475679	259355.824713	37.789645
1922.315806	259821.315882	37.794663
1924.567436	260294.512437	37.799680
1926.233651	260766.179752	37.804698
1928.115968	261244.568529	37.809716
1930.373621	261724.444772	37.814733
1931.936518	262200.879100	37.819751
1933.796279	262676.095650	37.824768
1935.594014	263164.176247	37.829786
1937.767677	263656.182801	37.834804
1939.742035	264147.485266	37.839821
1942.020954	264641.125003	37.844839
1944.289840	265124.503149	37.849856
1945.871121	265615.158145	37.854874
1947.850885	266091.902216	37.859892
1950.253991	266585.977083	37.864909
1952.419557	267069.675428	37.869927
1953.851339	267558.448043	37.874944
1956.013826	268048.268006	37.879962
1958.119613	268536.343964	37.884980
1960.315521	269029.815284	37.889997
1962.131718	269517.988656	37.895015
1964.347550	270002.767616	37.900032
1966.135603	270500.470394	37.905050
1968.226384	270978.155840	37.910068
1970.155554	271470.575483	37.915085
1972.056088	271975.166995	37.920103
1974.219399	272456.165976	37.925120
1976.408418	272952.376109	37.930138
1978.097363	273442.012459	37.935156
1980.156394	273940.934964	37.940173
1981.960553	274432.074636	37.945191
1984.162595	274925.052853	37.950208
1985.694192	275422.637021	37.955226
1987.671531	275920.146561	37.960244
1990.083615	276419.081996	37.965261
1991.809195	276927.782544	37.970279
1993.975471	277412.099262	37.975296
1995.655250	277925.809280	37.980314
1997.735433	278424.337697	37.985332
1999.678958	278931.981383	37.990349
2001.556250	279426.603519	37.995367
2003.875922	279930.524648	38.000384
2005.833580	280435.545691	38.005402
2008.069666	280942.780144	38.010420
2009.759248	281445.378707	38.015437
2012.156799	281941.533959	38.020455
2014.330558	282408.360588	38.025472
2015.933011	282893.874131	38.030490
2018.475819	283355.912537	38.035508
2020.280544	283825.869709	38.040525
2022.102162	284296.686362	38.045543
2024.283780	284774.859312	38.050560
2025.817362	285244.196606	38.055578
2027.889668	285724.797754	38.060596
2029.985909	286205.698220	38.065613
2031.634637	286684.156321	38.070631
2034.011409	287180.273156	38.075648
2035.830500	287676.683543	38.080666
2037.888570	288166.067556	38.085684
2039.761624	288659.976258	38.090701
2041.490033	289153.145027	38.095719
2043.795421	289670.321573	38.100736
2045.841364	290170.419191	38.105754
2047.663331	290678.222671	38.110772
2049.717166	291192.793028	38.115789
2051.342953	291709.362326	38.120807
2053.825286	292229.547200	38.125824
2055.874390	292758.615042	38.130842
2057.885121	293285.019918	38.135860
2060.232242	293814.846614	38.140877
2061.980516	294340.451868	38.145895
2063.946772	294860.354688	38.150912
2066.223841	295398.287920	38.155930
2067.907548	295936.824477	38.160948
2070.362605	296475.662805	38.165965
2072.282976	297023.730232	38.170983
2074.730038	297559.440366	38.176000
2076.738984	298104.160330	38.181018
2078.784242	298640.134407	38.186036
2081.098415	299172.886493	38.191053
2083.043568	299721.621228	38.196071
2085.677484	300265.540604	38.201088
2087.521736	300811.263571	38.206106
2089.949848	301352.645660	38.211124
2092.147832	301891.014970	38.216141
2094.154789	302434.847756	38.221159
2096.481647	302959.754463	38.226176
2098.716111	303507.022783	38.231194
2100.726983	304047.492959	38.236212
2103.071596	304589.149216	38.241229
2105.534595	305124.712841	38.246247
2107.458294	305662.825670	38.251264
2109.358260	306210.183293	38.256282
2111.768453	306731.828557	38.261300
2113.830694	307262.899135	38.266317
2115.918429	307805.669568	38.271335
2118.266866	308337.143165	38.276352
2120.412701	308879.693759	38.281370
2122.392828	309420.338036	38.286388
2124.773391	309966.677237	38.291405
2126.752316	310492.178985	38.296423
2128.833993	311033.912869	38.301440
2130.723885	311571.840060	38.306458
2133.031261	312111.167439	38.311476
2134.865452	312647.801145	38.316493
2137.088498	313199.552444	38.321511
2139.343507	313743.676243	38.326528
2140.870296	314285.275311	38.331546
2143.175523	314839.108463	38.336564
2145.635587	315379.605763	38.341581
2147.931392	315923.655738	38.346599
2150.126646	316461.395326	38.351616
2152.282377	317008.050150	38.356634
2154.565992	317546.071536	38.361652
2156.558191	318058.008201	38.366669
2158.719879	318579.130384	38.371687
2161.276723	319073.420294	38.376704
2162.989997	319592.247244	38.381722
2165.233620	320099.911925	38.386740
2167.677460	320600.633228	38.391757
2169.428615	321126.069036	38.396775
2171.677486	321645.908621	38.401792
2173.485362	322159.392974	38.406810
2175.648742	322689.826152	38.411828
2177.802305	323216.422591	38.416845
2179.567347	323751.584431	38.421863
2182.136517	324281.937221	38.426880
2184.087448	324823.838244	38.431898
2186.005154	325374.473924	38.436916
2188.544468	325914.897139	38.441933
2190.111959	326467.662630	38.446951
2192.371549	327021.984439	38.451968
2194.468389	327577.571982	38.456986
2196.811443	328141.897977	38.462004
2198.524249	328701.016480	38.467021
2200.829254	329275.619909	38.472039
2203.127510	329837.778863	38.477056
2205.427729	330419.505504	38.482074
2207.133321	330998.861794	38.487092
2209.456335	331583.923752	38.492109
2211.643498	332171.616799	38.497127
2213.987249	332757.323025	38.502144
2216.054519	333349.719738	38.507162
2218.104508	333956.455718	38.512180
2220.601329	334557.196354	38.517197
2222.841787	335161.475705	38.522215
2225.473445	335765.531309	38.527232
2227.620039	336362.577804	38.532250
2229.747258	336970.586639	38.537268
2232.728957	337565.679242	38.542285
2234.443999	338174.122728	38.547303
2237.038490	338770.991357	38.552320
2239.255330	339381.444415	38.557338
2241.308268	339996.942894	38.562356
2243.685231	340589.307781	38.567373
2245.598345	341204.154488	38.572391
2248.078586	341813.442851	38.577408
2250.591873	342425.154784	38.582426
2252.697452	343038.499930	38.587444
2255.136359	343646.528443	38.592461
2257.505687	344261.337286	38.597479
2259.823877	344875.207551	38.602496
2262.102274	345491.335195	38.607514
2264.177512	346103.021489	38.612532
2266.543002	346729.219426	38.617549
2268.380584	347339.735808	38.622567
2270.734467	347954.016366	38.627584
2273.358743	348572.634415	38.632602
2275.737208	349201.258011	38.637620
2277.949287	349826.829612	38.642637
2280.107701	350445.727150	38.647655
2282.599091	351054.588067	38.652672
2284.843769	351677.869635	38.657690
2286.950435	352306.392536	38.662708
2289.850307	352922.874290	38.667725
2291.583812	353546.391038	38.672743
2294.001359	354165.801972	38.677760
2296.331768	354784.583915	38.682778
2298.707653	355408.652483	38.687796
2301.285636	356027.629064	38.692813
2303.489357	356655.158300	38.697831
2306.189297	357248.596405	38.702848
2308.263862	357836.420349	38.707866
2310.438211	358428.659536	38.712884
2312.597910	358998.793643	38.717901
2314.895959	359591.807361	38.722919
2317.319844	360177.459326	38.727936
2319.829135	360764.889954	38.732954
2321.583126	361359.743236	38.737972
2324.087190	361943.554692	38.742989
2326.009627	362540.341243	38.748007
2328.570874	363143.989802	38.753024
2331.048874	363746.754824	38.758042
2332.894895	364359.102544	38.763060
2335.624966	364952.573012	38.768077
2337.527152	365576.891094	38.773095
2339.805659	366182.973900	38.778112
2342.133406	366789.952067	38.783130
2344.125041	367420.871036	38.788148
2346.965906	368044.967958	38.793165
2349.153042	368670.887136	38.798183
2351.523496	369302.929174	38.803200
2353.850564	369937.301043	38.808218
2356.200934	370564.758982	38.813236
2358.962358	371203.044664	38.818253
2361.243974	371845.912912	38.823271
2363.418901	372476.587720	38.828288
2366.147979	373127.500588	38.833306
2368.531517	373788.248248	38.838324
2370.656370	374425.338623	38.843341
2372.810856	375078.466058	38.848359
2375.498833	375729.261505	38.853376
2377.828228	376375.615193	38.858394
2380.208281	377041.627439	38.863412
2382.820328	377684.283485	38.868429
2385.214924	378357.216114	38.873447
2387.497699	379010.323830	38.878464
2390.143041	379670.433847	38.883482
2392.391748	380337.873820	38.888500
2395.004677	381000.752228	38.893517
2397.463498	381662.045398	38.898535
2400.083729	382323.881865	38.903552
2402.504957	382978.942676	38.908570
2404.652550	383647.650898	38.913588
2407.223088	384316.960123	38.918605
2409.925528	384983.926551	38.923623
2412.295817	385635.443282	38.928640
2414.895596	386299.534393	38.933658
2416.948855	386972.980625	38.938676
2419.870386	387633.035828	38.943693
2422.468495	388303.270896	38.948711
2424.702079	388968.025404	38.953728
2427.161030	389627.810686	38.958746
2429.615516	390287.785454	38.963764
2432.400657	390953.369638	38.968781
2434.759664	391621.265682	38.973799
2436.920291	392275.694940	38.978816
2439.751101	392932.889073	38.983834
2441.840592	393611.304849	38.988852
2444.673603	394265.960257	38.993869
2447.244509	394937.930116	38.998887
2449.759168	395597.829982	39.003904
2452.142957	396249.525222	39.008922
2454.444503	396911.838619	39.013940
2457.072106	397562.172023	39.018957
2459.446045	398225.254742	39.023975
2462.055842	398884.076658	39.028992
2464.547046	399539.735470	39.034010
2466.885580	400196.544877	39.039028
2469.293959	400842.051320	39.044045
2471.841394	401473.304676	39.049063
2474.266935	402095.366026	39.054080
2476.751647	402719.709733	39.059098
2479.445124	403336.809163	39.064116
2481.709822	403954.041768	39.069133
2484.053465	404581.509119	39.074151
2486.227984	405204.885732	39.079168
2488.951944	405830.513863	39.084186
2490.966137	406465.036182	39.089204
2493.340139	407103.943334	39.094221
2495.945751	407763.571138	39.099239
2498.187778	408411.994944	39.104256
2500.575221	409062.811165	39.109274
2502.751424	409724.058008	39.114292
2505.341070	410385.777633	39.119309
2507.610943	411052.042513	39.124327
2510.054998	411730.775068	39.129344
2512.534406	412407.382041	39.134362
2514.641336	413095.760366	39.139380
2517.096049	413793.054759	39.144397
2519.198461	414479.472509	39.149415
2521.764170	415189.754886	39.154432
2524.691643	415900.135368	39.159450
2526.569955	416614.594805	39.164468
2529.312092	417334.285986	39.169485
2531.754741	418062.413856	39.174503
2534.449698	418797.012636	39.179520
2536.965240	419520.680355	39.184538
2539.194600	420260.149968	39.189556
2541.917685	420997.414661	39.194573
2544.566394	421739.328769	39.199591
2547.170094	422485.810970	39.204608
2549.842710	423234.613901	39.209626
2552.070850	423978.201234	39.214644
2554.670986	424734.515128	39.219661
2557.150306	425497.255859	39.224679
2559.711443	426264.819714	39.229696
2562.127284	427024.991228	39.234714
2564.794789	427792.843272	39.239732
2567.459690	428567.151282	39.244749
2570.108349	429333.235600	39.249767
2572.753659	430113.065195	39.254784
2575.643318	430882.350084	39.259802
2577.763614	431665.150940	39.264820
2580.958840	432429.323297	39.269837
2583.746392	433207.001780	39.274855
2586.373546	433983.769567	39.279872
2589.012137	434748.311594	39.284890
2591.684631	435531.447529	39.289908
2594.198292	436301.070106	39.294925
2597.211835	437071.748179	39.299943
2599.558749	437844.129419	39.304960
2602.593769	438606.604063	39.309978
2605.129800	439387.554515	39.314996
2607.935792	440152.139689	39.320013
2610.804754	440919.673580	39.325031
2613.168485	441692.880568	39.330048
2615.892508	442450.063429	39.335066
2618.668196	443217.431662	39.340084
2621.533430	443986.731324	39.345101
2624.134919	444757.261522	39.350119
2626.402766	445512.136977	39.355136
2629.524988	446277.164840	39.360154
2631.926226	447028.424179	39.365172
2634.730487	447793.045850	39.370189
2637.418630	448552.196514	39.375207
2639.978059	449307.598432	39.380224
2642.509032	450051.850999	39.385242
2645.322852	450783.336075	39.390260
2647.855806	451496.837576	39.395277
2650.548684	452218.379998	39.400295
2653.322358	452938.265867	39.405312
2655.724835	453653.080554	39.410330
2658.125119	454377.933823	39.415348
2660.610678	455093.848017	39.420365
2663.330698	455825.575618	39.425383
2665.550970	456558.471864	39.430400
2668.257340	457300.969131	39.435418
2670.653067	458042.631013	39.440436
2673.192557	458787.325945	39.445453
2675.949685	459546.264394	39.450471
2678.454438	460308.046738	39.455488
2681.690955	461067.606793	39.460506
2684.210969	461835.141682	39.465524
2686.541962	462613.495077	39.470541
2689.403994	463373.534139	39.475559
2692.125532	464153.784163	39.480576
2694.658095	464921.904555	39.485594
2697.658717	465711.042761	39.490612
2699.706876	466498.537311	39.495629
2702.585872	467297.536346	39.500647
2705.398989	468099.898884	39.505664
2708.301742	468881.091471	39.510682
2710.809862	469701.628360	39.515700
2713.755586	470502.099992	39.520717
2716.436770	471303.491006	39.525735
2718.940835	472108.818048	39.530752
2721.960646	472913.975145	39.535770
2724.672889	473727.130263	39.540788
2727.257563	474546.383476	39.545805
2730.301406	475362.948811	39.550823
2732.862716	476187.740617	39.555840
2736.017022	476995.679514	39.560858
2738.389584	477828.611607	39.565876
2741.098729	478654.581869	39.570893
2743.830141	479477.733579	39.575911
2746.509007	480313.229168	39.580928
2749.491421	481150.959121	39.585946
2752.171213	481979.863593	39.590964
2754.989186	482823.955880	39.595981
2758.022900	483654.189088	39.600999
2760.397270	484498.124196	39.606016
2763.587543	485335.776025	39.611034
2766.661354	486170.630953	39.616052
2769.260204	487006.786805	39.621069
2772.331278	487835.101909	39.626087
2775.177612	488682.949114	39.631104
2777.994783	489513.548589	39.636122
2780.994710	490355.636155	39.641140
2784.073004	491199.537257	39.646157
2786.680040	492023.793122	39.651175
2789.198199	492864.929514	39.656192
2792.244699	493688.932129	39.661210
2795.295733	494522.885105	39.666228
2797.567757	495355.512956	39.671245
2800.808261	496196.265106	39.676263
2803.653328	497024.680112	39.681280
2806.312632	497858.634390	39.686298
2808.992044	498699.707296	39.691316
2812.130836	499532.439828	39.696333
2815.174987	500359.295181	39.701351
2817.699221	501194.467061	39.706368
2820.891913	502018.894965	39.711386
2823.587583	502849.566958	39.716404
2826.088232	503678.817061	39.721421
2828.834808	504497.142487	39.726439
2831.914968	505300.193630	39.731456
2834.721814	506082.425250	39.736474
2837.170843	506873.602686	39.741492
2840.001885	507670.325279	39.746509
2842.499490	508459.501017	39.751527
2845.086105	509264.100288	39.756544
2848.132069	510079.875433	39.761562
2851.089035	510890.280213	39.766580
2853.514868	511702.596277	39.771597
2856.312011	512508.307417	39.776615
2858.981321	513337.586083	39.781632
2861.869022	514155.999834	39.786650
2864.371698	514997.868250	39.791668
2867.110210	515836.225726	39.796685
2869.716837	516681.211306	39.801703
2872.246204	517547.830122	39.806720
2875.019765	518405.442097	39.811738
2877.819920	519267.838606	39.816756
2880.655459	520153.052781	39.821773
2883.699323	521035.561882	39.826791
2886.260168	521929.282340	39.831808
2888.980491	522817.635135	39.836826
2891.986164	523719.790028	39.841844
2894.694488	524629.746426	39.846861
2897.782995	525523.872533	39.851879
2900.778102	526451.750723	39.856896
2903.632610	527362.071072	39.861914
2906.757318	528284.828701	39.866932
2909.494584	529221.891713	39.871949
2912.610856	530136.026474	39.876967
2915.732833	531077.690936	39.881984
2918.481958	531999.825019	39.887002
2921.610017	532938.650527	39.892020
2924.350399	533867.714995	39.897037
2928.234544	534806.144250	39.902055
2930.587845	535742.651358	39.907072
2933.698137	536683.954732	39.912090
2937.036253	537625.460762	39.917108
2939.569295	538556.521583	39.922125
2942.425420	539501.052760	39.927143
2945.551477	540443.413979	39.932160
2948.926577	541387.331521	39.937178
2952.007690	542335.610719	39.942196
2954.807600	543283.972945	39.947213
2957.959600	544239.455521	39.952231
2960.906539	545180.724127	39.957248
2964.007497	546120.797325	39.962266
2967.182925	547062.554518	39.967284
2969.939343	548014.071342	39.972301
2973.324408	548960.038988	39.977319
2976.065696	549914.192150	39.982336
2979.400580	550851.088571	39.987354
2982.563765	551795.841010	39.992372
2985.317287	552740.846635	39.997389
2988.712865	553670.149776	40.002407
2991.734406	554610.406770	40.007424
2994.812566	555547.874990	40.012442
2997.738292	556482.991270	40.017460
3000.544634	557433.286665	40.022477
3003.814724	558358.868733	40.027495
3006.843918	559308.842619	40.032512
3009.331423	560241.506074	40.037530
3012.771709	561175.805106	40.042548
3015.763390	562122.769461	40.047565
3019.102950	563052.229960	40.052583
3021.899037	563995.324087	40.057600
3024.933188	564927.664348	40.062618
3028.032289	565850.787816	40.067636
3030.743693	566757.289392	40.072653
3034.060731	567645.652997	40.077671
3037.045471	568530.997730	40.082688
3039.867022	569424.039151	40.087706
3042.676269	570311.749465	40.092724
3045.511160	571205.567545	40.097741
3048.940537	572107.004212	40.102759
3051.819690	573010.374510	40.107776
3054.722914	573917.690846	40.112794
3057.890290	574819.027223	40.117812
3060.808500	575738.302891	40.122829
3063.744885	576647.373234	40.127847
3066.382462	577568.266344	40.132864
3069.500302	578491.068831	40.137882
3072.611948	579424.989537	40.142900
3075.273707	580371.302644	40.147917
3078.384352	581306.936872	40.152935
3081.437902	582268.687228	40.157952
3084.277548	583218.964134	40.162970
3087.381683	584181.357984	40.167988
3090.464273	585154.709511	40.173005
3093.563559	586119.457473	40.178023
3096.677433	587099.616049	40.183040
3099.812797	588086.358036	40.188058
3102.812135	589073.392247	40.193076
3105.933978	590070.097734	40.198093
3109.452513	591055.980559	40.203111
3112.401626	592048.189262	40.208128
3115.657748	593046.076479	40.213146
3119.071590	594045.206180	40.218164
3122.093348	595035.999876	40.223181
3125.202246	596039.318783	40.228199
3128.547152	597049.875686	40.233216
3131.525192	598053.544208	40.238234
3134.486783	599063.689205	40.243252
3137.800567	600075.540944	40.248269
3141.008936	601084.217181	40.253287
3144.243276	602111.575471	40.258304
3147.298496	603121.500237	40.263322
3151.021556	604138.133699	40.268340
3153.810677	605175.301935	40.273357
3157.118408	606191.820712	40.278375
3160.514858	607214.289016	40.283392
3163.877796	608241.774351	40.288410
3166.618091	609266.766992	40.293428
3170.050456	610298.306069	40.298445
3173.093816	611312.105497	40.303463
3176.238752	612356.958819	40.308480
3179.363702	613381.761182	40.313498
3182.858052	614425.962325	40.318516
3185.932626	615466.783707	40.323533
3189.238579	616489.768209	40.328551
3192.024980	617528.042230	40.333568
3195.487181	618565.456633	40.338586
3199.026552	619607.158717	40.343604
3201.859403	620650.227180	40.348621
3205.198868	621687.464489	40.353639
3208.404541	622725.074242	40.358656
3211.655294	623773.919588	40.363674
3215.278127	624801.766691	40.368692
3218.484286	625841.923737	40.373709
3221.975396	626881.133400	40.378727
3224.958413	627926.918757	40.383744
3228.069494	628958.146367	40.388762
3231.613513	629997.641966	40.393780
3234.796223	631037.444384	40.398797
3237.537831	632071.774604	40.403815
3240.915705	633091.519922	40.408832
3243.937013	634094.901045	40.413850
3247.563856	635086.355986	40.418868
3250.680749	636078.299654	40.423885
3253.943696	637053.855363	40.428903
3257.098536	638052.989806	40.433920
3259.956599	639051.577509	40.438938
3263.473352	640045.369829	40.443956
3266.721865	641038.361846	40.448973
3269.715599	642041.724675	40.453991
3272.737077	643051.019318	40.459008
3275.811745	644070.678056	40.464026
3279.208776	645084.945271	40.469044
3282.147970	646114.044894	40.474061
3285.251749	647145.604953	40.479079
3288.931011	648188.529793	40.484096
3291.595063	649229.370160	40.489114
3294.991646	650279.750225	40.494132
3298.481585	651349.041279	40.499149
3301.509298	652390.239380	40.504167
3305.000985	653462.342168	40.509184
3307.801291	654539.225255	40.514202
3310.929260	655622.960408	40.519220
3314.349556	656710.114048	40.524237
3317.379715	657810.359196	40.529255
3321.062478	658906.588317	40.534272
3323.716424	660018.448222	40.539290
3327.377343	661133.698990	40.544308
3330.589561	662261.489449	40.549325
3334.162757	663380.278667	40.554343
3337.593865	664491.346691	40.559360
3340.796656	665631.832626	40.564378
3344.508405	666755.778634	40.569396
3347.910738	667890.637951	40.574413
3351.147543	669034.691243	40.579431
3354.803587	670170.479711	40.584448
3357.893374	671313.386397	40.589466
3361.595545	672450.583585	40.594484
3364.691233	673615.089110	40.599501
3368.214570	674754.721144	40.604519
3371.879301	675913.875059	40.609536
3374.802995	677069.875462	40.614554
3378.648849	678224.337453	40.619572
3382.106001	679378.769047	40.624589
3385.230728	680538.774737	40.629607
3388.883937	681695.218599	40.634624
3391.983832	682867.998953	40.639642
3395.420307	684031.137119	40.644660
3398.994407	685202.595537	40.649677
3402.557437	686369.783579	40.654695
3406.165651	687529.267649	40.659712
3409.521691	688711.180196	40.664730
3412.991957	689874.306684	40.669748
3416.300712	691053.486908	40.674765
3419.956321	692221.885670	40.679783
3423.358355	693388.734351	40.684800
3426.851898	694562.756489	40.689818
3430.404175	695730.711116	40.694836
3433.915741	696903.774927	40.699853
3437.147284	698074.249391	40.704871
3440.914022	699239.720075	40.709888
3444.003011	700412.930309	40.714906
3447.641530	701592.038612	40.719924
3451.029968	702755.764079	40.724941
3454.469130	703930.127741	40.729959
3457.982992	705109.125745	40.734976
3461.355096	706294.079385	40.739994
3464.826399	707449.480652	40.745012
3468.016986	708618.607179	40.750016
3471.549321	709733.497978	40.755021
3475.243581	710795.052148	40.760026
3478.204606	711787.057485	40.765031
3481.489836	712726.932396	40.770036
3484.511578	713604.915705	40.775040
3487.228236	714411.109583	40.780045
3490.279244	715134.116976	40.785050
3493.015180	715805.023221	40.790055
3495.808687	716394.659993	40.795060
3498.425800	716930.613110	40.800064
3500.575329	717406.195053	40.805069
3503.126058	717810.410825	40.810074
3505.319828	718163.482312	40.815079
3507.114551	718450.693253	40.820084
3509.052080	718701.370103	40.825088
3510.810894	718888.739737	40.830093
3512.546022	719014.268625	40.835098
3513.775228	719112.901540	40.840103
3515.457694	719144.660101	40.845108
3516.725058	719162.948698	40.850112
3517.828224	719132.516656	40.855117
3519.154842	719053.200390	40.860122
3520.409780	718958.918454	40.865127
3521.623603	718811.528574	40.870132
3522.411782	718654.188315	40.875136
3523.451039	718442.398263	40.880141
3524.115213	718211.718888	40.885146
3524.605676	717966.331257	40.890151
3525.635137	717681.118560	40.895156
3526.477346	717397.464647	40.900160
3526.446262	717077.189274	40.905165
3527.323678	716725.153582	40.910170
3527.800451	716388.696180	40.915175
3528.147089	716020.546489	40.920180
3528.341680	715653.249125	40.925184
3528.943760	715250.196339	40.930189
3529.506501	714848.222309	40.935194
3529.187129	714439.328631	40.940199
3529.881572	714003.899308	40.945204
3530.114590	713566.935623	40.950208
3530.229375	713126.346127	40.955213
3530.348560	712676.799777	40.960218
3530.576601	712223.836703	40.965223
3531.008223	711744.906808	40.970228
3530.555104	711283.965056	40.975232
3530.567336	710812.398005	40.980237
3530.927896	710328.336795	40.985242
3531.013192	709870.307633	40.990247
3531.049759	709375.274113	40.995252
3531.009079	708875.656745	41.000256
3530.699132	708398.547786	41.005261
3530.864740	707898.938731	41.010266
3530.827332	707410.060499	41.015271
3530.896258	706909.813880	41.020276
3530.923920	706423.699566	41.025280
3530.649662	705913.121157	41.030285
3530.810773	705407.904586	41.035290
3530.817119	704922.702549	41.040295
3530.713348	704410.467247	41.045300
3530.604841	703917.180053	41.050304
3530.228926	703408.606602	41.055309
3530.301845	702906.239426	41.060314
3530.408092	702408.955596	41.065319
3530.356963	701902.625465	41.070324
3530.191098	701408.956776	41.075328
3529.681098	700899.215042	41.080333
3529.809159	700402.558538	41.085338
3529.428239	699907.796673	41.090343
3529.430519	699408.171968	41.095348
3529.124310	698926.414839	41.100352
3529.339445	698433.509527	41.105357
3529.155631	697930.102979	41.110362
3528.989689	697446.700440	41.115367
3528.904547	696946.800965	41.120372
3528.861241	696453.479292	41.125376
3528.739433	695964.021523	41.130381
3528.452637	695476.403753	41.135386
3528.166826	695002.335319	41.140391
3528.070858	694517.865780	41.145396
3527.776189	694039.569745	41.150400
3527.510394	693564.277229	41.155405
3527.299537	693078.653866	41.160410
3527.122468	692620.954385	41.165415
3527.163763	692153.445171	41.170420
3526.743025	691688.325793	41.175424
3526.447827	691222.614246	41.180429
3526.543584	690764.127863	41.185434
3526.205935	690320.566597	41.190439
3526.061332	689850.629108	41.195444
3526.030671	689406.822805	41.200448
3525.861854	688958.538600	41.205453
3525.869613	688504.579359	41.210458
3525.648062	688068.850444	41.215463
3525.631219	687614.900221	41.220468
3525.339354	687184.366172	41.225472
3524.876100	686748.712916	41.230477
3524.921764	686306.632952	41.235482
3524.477335	685878.749960	41.240487
3524.551141	685447.973523	41.245492
3524.420153	685023.134885	41.250496
3524.061441	684601.052248	41.255501
3524.200553	684174.635833	41.260506
3523.803370	683761.482849	41.265511
3523.780310	683338.539519	41.270516
3523.529488	682922.336733	41.275520
3523.357747	682504.657781	41.280525
3523.453721	682104.047388	41.285530
3522.841101	681690.089227	41.290535
3522.657401	681290.535234	41.295540
3522.665885	680881.916909	41.300544
3522.424621	680486.222444	41.305549
3522.277226	680083.970056	41.310554
3522.209783	679700.168137	41.315559
3522.341271	679298.383457	41.320564
3521.981254	678912.305391	41.325568
3521.736566	678529.978566	41.330573
3521.370878	678130.267650	41.335578
3521.320182	677755.748892	41.340583
3521.250477	677378.975910	41.345588
3521.001714	677011.983619	41.350592
3520.688757	676633.725583	41.355597
3520.823423	676275.510934	41.360602
3520.383269	675903.971611	41.365607
3520.213188	675541.991483	41.370612
3520.152467	675177.437492	41.375616
3520.069994	674829.170766	41.380621
3519.968685	674460.408833	41.385626
3519.891391	674111.815453	41.390631
3519.783905	673750.453372	41.395636
3519.286624	673408.931360	41.400640
3519.171935	673049.986008	41.405645
3519.019345	672704.991742	41.410650
3518.497585	672370.165955	41.415655
3518.899394	672027.249013	41.420660
3518.672566	671704.515683	41.425664
3518.334529	671367.878933	41.430669
3518.367567	671020.797938	41.435674
3518.260577	670720.149376	41.440679
3518.179306	670384.781510	41.445684
3517.865882	670062.504894	41.450688
3517.427218	669742.681445	41.455693
3517.324226	669424.537301	41.460698
3516.780469	669131.889295	41.465703
3517.072679	668825.579060	41.470708
3517.240047	668515.888068	41.475712
3516.899788	668215.647264	41.480717
3516.640796	667896.879086	41.485722
3516.604402	667602.703767	41.490727
3516.912570	667300.980508	41.495732
3516.469223	667007.552188	41.500736
3516.124343	666708.761063	41.505741
3516.460055	666411.394873	41.510746
3516.006499	666122.979425	41.515751
3516.212599	665835.344560	41.520756
3515.879647	665545.943952	41.525760
3515.702662	665268.333096	41.530765
3515.753786	664991.923920	41.535770
3515.286838	664713.346912	41.540775
3515.518206	664427.960748	41.545780
3515.298892	664151.072952	41.550784
3514.884709	663878.849833	41.555789
3514.781175	663615.150570	41.560794
3514.736568	663348.789612	41.565799
3514.726470	663082.116185	41.570804
3514.816188	662814.570564	41.575808
3514.302367	662555.051903	41.580813
3514.772473	662289.075901	41.585818
3514.477116	662033.599558	41.590823
3514.301321	661766.617630	41.595828
3513.799911	661515.104365	41.600832
3513.646010	661259.733994	41.605837
3513.761909	661013.646197	41.610842
3513.880118	660780.729172	41.615847
3513.728585	660525.039562	41.620852
3513.480419	660290.573836	41.625856
3513.399731	660044.893190	41.630861
3513.351906	659802.046322	41.635866
3513.125668	659555.279056	41.640871
3512.675803	659313.933944	41.645876
3513.066754	659083.876689	41.650880
3513.049587	658862.568071	41.655885
3512.730820	658621.982996	41.660890
3512.339081	658402.073632	41.665895
3512.481050	658169.439651	41.670900
3512.148970	657950.009548	41.675904
3512.038586	657732.984554	41.680909
3512.091583	657516.177476	41.685914
3511.813073	657307.758894	41.690919
3511.733903	657091.163907	41.695924
3511.666381	656869.668640	41.700928
3511.352210	656663.639075	41.705933
3511.745944	656449.298943	41.710938
3511.465660	656262.530851	41.715943
3511.385235	656043.915437	41.720948
3511.712959	655844.604490	41.725952
3510.945085	655647.767304	41.730957
3511.329315	655431.808441	41.735962
3510.926192	655247.138841	41.740967
3510.849258	655048.078206	41.745972
3510.937833	654850.584505	41.750976
3511.017965	654660.979649	41.755981
3510.905698	654460.214811	41.760986
3510.577486	654274.815387	41.765991
3510.467214	654077.239071	41.770996
3510.422841	653888.988509	41.776000
3510.364868	653705.981399	41.781005
3510.499416	653519.892144	41.786010
3510.113121	653335.883307	41.791015
3510.459761	653143.208264	41.796020
3510.218485	652958.469167	41.801024
3509.937218	652782.025765	41.806029
3510.135472	652599.105835	41.811034
3509.860174	652420.157206	41.816039
3509.619634	652253.589156	41.821044
3510.118665	652074.506700	41.826048
3509.876234	651903.286926	41.831053
3509.897880	651712.086468	41.836058
3509.413374	651553.990205	41.841063
3509.334940	651367.995593	41.846068
3509.304685	651209.019598	41.851072
3509.168610	651044.662406	41.856077
3509.272720	650873.967374	41.861082
3509.124730	650720.798888	41.866087
3508.832728	650545.266880	41.871092
3508.948067	650399.395116	41.876096
3509.063694	650242.628184	41.881101
3509.176473	650079.063521	41.886106
3508.845885	649921.465638	41.891111
3508.847181	649763.061025	41.896116
3508.488445	649607.911375	41.901120
3508.880933	649451.336262	41.906125
3508.842194	649294.429977	41.911130
3508.463834	649139.925944	41.916135
3508.220063	648988.395796	41.921140
3508.323778	648833.008004	41.926144
3508.007232	648700.226061	41.931149
3508.241029	648545.162200	41.936154
3508.401847	648408.499531	41.941159
3508.233991	648256.346082	41.946164
3508.132613	648110.676579	41.951168
3507.840935	647965.386175	41.956173
3507.989063	647832.916017	41.961178
3507.965985	647699.022888	41.966183
3508.177413	647550.394845	41.971188
3507.816279	647411.305553	41.976192
3507.826932	647270.103783	41.981197
3507.979241	647135.874363	41.986202
3507.734205	647006.856980	41.991207
3507.873404	646859.480238	41.996212
3507.552678	646726.173045	42.001216
3507.493261	646586.872688	42.006221
3507.813914	646463.303584	42.011226
3507.552029	646327.132177	42.016231
3507.438915	646192.384070	42.021236
3507.770373	646059.960364	42.026240
3507.396783	645931.250333	42.031245
3507.608463	645800.542601	42.036250
3507.275816	645675.821766	42.041255
3507.268171	645536.198438	42.046260
3507.377924	645409.901684	42.051264
3506.940012	645296.941609	42.056269
3507.465523	645154.525568	42.061274
3507.028583	645039.112789	42.066279
3507.324678	644905.030001	42.071284
3507.257417	644784.154004	42.076288
3506.915849	644654.322557	42.081293
3506.777884	644530.755424	42.086298
3506.665147	644420.931752	42.091303
3506.722037	644303.479344	42.096308
3506.760199	644187.928584	42.101312
3506.590933	644076.160577	42.106317
3506.737723	643958.789365	42.111322
3506.462929	643851.336190	42.116327
3506.528067	643737.075846	42.121332
3506.590957	643620.664557	42.126336
3506.207160	643511.025713	42.131341
3506.389859	643387.291824	42.136346
3506.239369	643293.162755	42.141351
3506.403828	643186.280200	42.146356
3506.193543	643069.007563	42.151360
3506.249689	642958.240195	42.156365
3506.212621	642843.586629	42.161370
3506.218288	642751.777036	42.166375
3506.080719	642636.437631	42.171380
3506.147940	642531.114400	42.176384
3506.261420	642427.932743	42.181389
3506.178382	642311.680561	42.186394
3506.129382	642218.374961	42.191399
3505.991338	642108.330467	42.196404
3505.842722	641997.636417	42.201408
3505.794009	641914.029668	42.206413
3506.095478	641804.809645	42.211418
3505.687738	641705.307267	42.216423
3506.235093	641607.897013	42.221428
3505.667938	641503.167822	42.226432
3505.650419	641408.249281	42.231437
3506.037430	641305.711382	42.236442
3505.744515	641201.534056	42.241447
3505.740825	641116.713069	42.246452
3505.808187	641020.326569	42.251456
3505.880542	640918.336777	42.256461
3505.767097	640811.225096	42.261466
3505.723686	640723.506559	42.266471
3505.544937	640624.806192	42.271476
3505.673100	640526.504445	42.276480
3505.708214	640432.568510	42.281485
3505.898258	640337.905950	42.286490
3505.511024	640238.385934	42.291495
3505.335109	640146.832969	42.296500
3505.595678	640055.457353	42.301504
3505.235285	639961.682318	42.306509
3505.539803	639866.796480	42.311514
3505.176061	639773.520469	42.316519
3505.136214	639682.691238	42.321524
3504.963836	639600.486553	42.326528
3504.963893	639516.852214	42.331533
3505.185470	639431.279887	42.336538
3505.282141	639361.084057	42.341543
3505.438945	639269.718560	42.346548
3505.302828	639167.545649	42.351552
3505.039417	639086.652443	42.356557
3505.104215	638998.401119	42.361562
3505.007954	638918.529538	42.366567
3504.830975	638824.013573	42.371572
3504.943379	638748.608464	42.376576
3504.810227	638677.895580	42.381581
3504.886713	638581.084503	42.386586
3504.789242	638510.564693	42.391591
3504.831228	638428.115223	42.396596
3504.684338	638343.244920	42.401600
3504.385613	638270.105225	42.406605
3504.811428	638198.646599	42.411610
3504.645243	638124.383434	42.416615
3504.364676	638042.034059	42.421620
3504.535769	637968.564670	42.426624
3504.494842	637908.787510	42.431629
3504.670472	637807.200123	42.436634
3504.677653	637741.860842	42.441639
3504.800300	637666.296054	42.446644
3504.606537	637596.886527	42.451648
3504.513114	637524.808387	42.456653
3504.175822	637449.968204	42.461658
3504.581310	637368.450998	42.466663
3504.671379	637291.588031	42.471668
3504.393615	637232.446368	42.476672
3504.064229	637169.160204	42.481677
3505.099256	637065.922964	42.486682
3505.150079	636999.170889	42.491687
3504.678577	636921.447087	42.496692
3503.976644	636859.821488	42.501696
3504.317579	636782.963444	42.506701
3505.042978	636694.233353	42.511706
3504.463756	636640.491669	42.516711
3504.308861	636559.911038	42.521716
3504.601297	636480.056637	42.526720
3504.185979	636409.374736	42.531725
3504.744928	636344.386042	42.536730
3504.738488	636267.981717	42.541735
3504.779033	636193.270341	42.546740
3504.398086	636123.131232	42.551744
3504.252446	636040.293367	42.556749
3504.314570	635966.877784	42.561754
3504.407056	635906.616749	42.566759
3504.249532	635833.286455	42.571764
3504.546376	635760.481239	42.576768
3504.210065	635698.538293	42.581773
3504.290518	635627.419098	42.586778
3503.671364	635559.016778	42.591783
3504.194914	635493.077842	42.596788
3504.284736	635440.120416	42.601792
3504.296224	635369.561269	42.606797
3504.567351	635287.349302	42.611802
3503.959564	635228.851095	42.616807
3504.143774	635153.808329	42.621812
3504.674395	635082.711319	42.626816
3504.207451	635030.444062	42.631821
3503.844728	634958.842862	42.636826
3503.820496	634889.787636	42.641831
3504.022144	634823.947556	42.646836
3503.926565	634763.310547	42.651840
3503.663344	634707.304859	42.656845
3504.413491	634639.571648	42.661850
3504.106906	634577.366908	42.666855
3504.211478	634506.636448	42.671860
3504.094955	634450.605208	42.676864
3503.763042	634386.251556	42.681869
3503.969031	634312.200060	42.686874
3504.108671	634247.817896	42.691879
3503.764020	634196.226948	42.696884
3503.679103	634142.641124	42.701888
3503.547519	634077.401762	42.706893
3503.991015	634015.420400	42.711898
3504.023875	633957.910528	42.716903
3503.911263	633893.667845	42.721908
3504.057672	633828.180928	42.726912
3503.625836	633782.207701	42.731917
3503.814484	633718.414782	42.736922
3504.088014	633643.997083	42.741927
3504.253819	633582.459310	42.746932
3504.211950	633523.457882	42.751936
3503.736583	633459.772806	42.756941
3503.694457	633403.123090	42.761946
3503.586949	633346.834195	42.766951
3503.631486	633292.221670	42.771956
3503.833863	633235.080299	42.776960
3503.764523	633189.595293	42.781965
3503.750849	633124.480712	42.786970
3503.674607	633068.535531	42.791975
3503.767501	633002.751958	42.796980
3503.723763	632939.393007	42.801985
3503.732329	632891.891773	42.806989
3503.573468	632826.148578	42.811994
3503.311556	632776.989590	42.816999
3503.535152	632722.995286	42.822004
3503.903399	632673.381599	42.827009
3503.713901	632606.340676	42.832013
3503.907420	632543.991376	42.837018
3503.551031	632498.750892	42.842023
3503.763851	632436.898321	42.847028
3503.720980	632374.186527	42.852033
3503.648539	632328.498077	42.857037
3503.798293	632264.152111	42.862042
3503.734719	632208.951094	42.867047
3503.581907	632156.267302	42.872052
3504.048789	632082.707678	42.877057
3503.809338	632035.794061	42.882061
3503.643564	631976.604120	42.887066
3503.503430	631918.110423	42.892071
3503.705236	631857.257404	42.897076
3503.742762	631803.789616	42.902081
3503.886291	631743.646353	42.907085
3504.127036	631685.238773	42.912090
3504.085303	631630.281411	42.917095
3503.958414	631577.540388	42.922100
3503.838905	631511.982717	42.927105
3503.992100	631448.632383	42.932109
3503.862634	631376.918182	42.937114
3503.998615	631328.537867	42.942119
3503.885148	631257.420937	42.947124
3504.071837	631201.822972	42.952129
3503.853837	631145.940973	42.957133
3504.130047	631076.610868	42.962138
3503.967558	631015.712895	42.967143
3503.923352	630954.044150	42.972148
3503.876584	630884.165259	42.977153
3503.477096	630824.156291	42.982157
3503.752112	630771.995820	42.987162
3503.368112	630724.799800	42.992167
3503.769314	630667.411465	42.997172
3503.812012	630610.682656	43.002177
3503.646701	630566.153321	43.007181
3503.642771	630498.367494	43.012186
3503.711467	630445.388319	43.017191
3503.553520	630387.740153	43.022196
3503.850546	630336.875587	43.027201
3503.454606	630286.525486	43.032205
3503.634971	630217.305664	43.037210
3503.444708	630168.423071	43.042215
3503.369162	630113.713703	43.047220
3503.404048	630051.826390	43.052225
3503.401325	630017.181052	43.057229
3503.524485	629964.040290	43.062234
3503.360974	629921.360405	43.067239
3503.212774	629864.959450	43.072244
3503.570214	629823.545137	43.077249
3503.333899	629767.308383	43.082253
3503.543917	629709.045136	43.087258
3503.499580	629669.799277	43.092263
3503.358741	629604.533679	43.097268
3503.529750	629553.736183	43.102273
3503.481042	629499.870384	43.107277
3503.394764	629451.618236	43.112282
3503.462139	629399.985906	43.117287
3503.453690	629340.354692	43.122292
3503.582652	629296.071932	43.127297
3503.392974	629241.727351	43.132301
3503.476166	629178.224730	43.137306
3503.622017	629132.536535	43.142311
3503.403180	629070.735367	43.147316
3503.340729	629033.442897	43.152321
3503.284127	628986.635800	43.157325
3503.099425	628930.636453	43.162330
3503.356090	628889.936102	43.167335
3503.559630	628828.414422	43.172340
3503.803044	628778.051928	43.177345
3503.659993	628727.903096	43.182349
3503.721076	628679.923587	43.187354
3503.383343	628624.398494	43.192359
3503.724184	628574.469637	43.197364
3503.698208	628512.633436	43.202369
3503.523162	628467.495992	43.207373
3503.456648	628412.175464	43.212378
3503.347878	628354.207677	43.217383
3503.506426	628302.354686	43.222388
3503.476052	628245.875624	43.227393
3503.205845	628190.988108	43.232397
3503.557300	628138.701931	43.237402
3503.196862	628098.951519	43.242407
3502.942509	628045.863355	43.247412
3503.308681	627992.522445	43.252417
3503.205531	627956.434721	43.257421
3503.347531	627896.970911	43.262426
3503.117601	627854.594107	43.267431
3503.094682	627805.122194	43.272436
3503.332475	627755.757320	43.277441
3503.207803	627713.713149	43.282445
3503.352640	627665.965649	43.287450
3503.382156	627621.692298	43.292455
3503.159976	627572.802995	43.297460
3503.255598	627520.205393	43.302465
3503.054163	627465.703425	43.307469
3503.184543	627416.655151	43.312474
3503.096750	627376.256165	43.317479
3503.203789	627329.565042	43.322484
3503.133053	627288.812360	43.327489
3503.068084	627257.623738	43.332493
3503.286852	627198.193457	43.337498
3503.126548	627147.388977	43.342503
3502.743541	627118.305631	43.347508
3503.494501	627058.786876	43.352513
3503.219041	627029.835808	43.357517
3503.180673	626973.050828	43.362522
3503.322832	626928.705956	43.367527
3503.061348	626875.312643	43.372532
3503.038639	626822.580856	43.377537
3502.724351	626787.425428	43.382541
3503.200323	626738.317088	43.387546
3503.485245	626694.999439	43.392551
3503.024952	626656.211649	43.397556
3503.067020	626600.763653	43.402561
3503.037963	626556.996358	43.407565
3503.249810	626509.032307	43.412570
3503.253352	626461.953780	43.417575
3502.843508	626430.068322	43.422580
3502.910370	626362.544929	43.427585
3502.712075	626333.028333	43.432589
3503.085082	626290.896541	43.437594
3503.216831	626249.906189	43.442599
3503.299688	626207.170787	43.447604
3503.330897	626154.777409	43.452609
3503.219422	626118.885174	43.457613
3503.451508	626055.289307	43.462618
3503.357645	626021.797925	43.467623
3503.002209	625975.127004	43.472628
3502.980829	625927.899975	43.477633
3502.936406	625877.020268	43.482637
3503.195742	625833.903692	43.487642
3502.802015	625789.692488	43.492647
3502.832420	625747.013977	43.497652
3503.478747	625703.532588	43.502657
3503.388008	625658.118919	43.507661
3503.532537	625598.090933	43.512666
3503.089610	625567.961403	43.517671
3503.323240	625523.595633	43.522676
3503.419023	625473.041515	43.527681
3502.970069	625434.397681	43.532685
3503.278082	625373.740444	43.537690
3503.389377	625328.442349	43.542695
3503.223536	625276.878561	43.547700
3503.200499	625230.199704	43.552705
3503.329754	625186.450805	43.557709
3503.315664	625127.197658	43.562714
3503.162818	625089.605750	43.567719
3503.185863	625035.855826	43.572724
3503.523692	624979.699530	43.577729
3503.231448	624932.061936	43.582733
3503.147104	624888.397110	43.587738
3503.226064	624844.705197	43.592743
3503.046113	624797.198771	43.597748
3503.078173	624745.148996	43.602753
3503.209075	624709.362372	43.607757
3503.481916	624670.947481	43.612762
3503.469094	624613.694949	43.617767
3503.452252	624561.552160	43.622772
3503.579789	624513.542982	43.627777
3503.238661	624466.111743	43.632781
3503.410314	624421.851819	43.637786
3503.337130	624374.025371	43.642791
3503.043953	624317.017828	43.647796
3503.522334	624260.333682	43.652801
3503.270863	624218.897784	43.657805
3503.322088	624165.589705	43.662810
3503.340374	624125.912375	43.667815
3503.337539	624080.327260	43.672820
3503.769156	624015.734639	43.677825
3503.366872	623978.280133	43.682829
3503.554408	623913.877407	43.687834
3503.344892	623874.236687	43.692839
3503.650038	623819.883150	43.697844
3503.939822	623767.235124	43.702849
3503.522463	623719.612768	43.707853
3503.518142	623656.342227	43.712858
3503.347206	623615.441791	43.717863
3503.441206	623559.418456	43.722868
3503.411418	623504.667651	43.727873
3503.146614	623458.922686	43.732877
3503.352045	623410.545074	43.737882
3503.276751	623367.223261	43.742887
3503.231523	623309.067372	43.747892
3503.361145	623264.108247	43.752897
3503.451620	623211.790941	43.757901
3503.445557	623154.429337	43.762906
3503.255835	623119.441741	43.767911
3503.165925	623070.159395	43.772916
3503.565322	623021.046689	43.777921
3503.180424	622980.129000	43.782925
3503.114192	622929.940324	43.787930
3503.299906	622886.272972	43.792935
3503.198138	622846.460415	43.797940
3503.176416	622791.253760	43.802945
3502.934661	622744.249458	43.807949
3503.081925	622692.822087	43.812954
3503.013413	622653.604547	43.817959
3503.293160	622615.181195	43.822964
3503.254055	622562.781896	43.827969
3503.047941	622514.067274	43.832973
3503.217201	622451.863300	43.837978
3503.449752	622404.879566	43.842983
3502.987896	622364.874061	43.847988
3503.190001	622319.247732	43.852993
3502.731713	622278.740295	43.857997
3503.362280	622221.870063	43.863002
3502.921643	622179.455436	43.868007
3502.502196	622143.500470	43.873012
3502.949764	622100.488242	43.878017
3502.575295	622082.663091	43.883021
3502.813348	622025.054850	43.888026
3503.006147	621995.161266	43.893031
3502.740679	621953.368237	43.898036
3503.134449	621910.163702	43.903041
3502.910009	621872.221631	43.908045
3503.091302	621824.792886	43.913050
3502.902710	621788.748594	43.918055
3503.134442	621738.755812	43.923060
3503.374764	621693.070443	43.928065
3503.257223	621655.260312	43.933069
3503.234569	621596.891068	43.938074
3503.319212	621560.600569	43.943079
3502.685946	621513.304688	43.948084
3503.406155	621457.217375	43.953089
3502.776167	621421.294701	43.958093
3503.105350	621368.428078	43.963098
3503.030997	621335.119326	43.968103
3502.949645	621295.748661	43.973108
3502.761219	621251.284547	43.978113
3502.936102	621216.180602	43.983117
3503.283330	621173.882742	43.988122
3503.019013	621126.424158	43.993127
3503.247468	621086.951575	43.998132
3503.252344	621035.239151	44.003137
3502.966748	620999.759410	44.008141
3503.429476	620938.350236	44.013146
3503.144194	620902.068384	44.018151
3502.838448	620856.920460	44.023156
3503.111240	620808.770669	44.028161
3502.750193	620766.036731	44.033165
3502.926367	620713.943782	44.038170
3503.168780	620690.252048	44.043175
3503.208360	620640.536424	44.048180
3503.112253	620599.010925	44.053185
3502.596977	620553.345052	44.058189
3503.145046	620506.100660	44.063194
3503.322173	620464.329179	44.068199
3502.953420	620425.754383	44.073204
3503.143263	620386.285621	44.078209
3502.966280	620345.073147	44.083213
3503.009123	620300.216247	44.088218
3502.912491	620253.277444	44.093223
3503.124670	620213.954712	44.098228
3503.237185	620173.996800	44.103233
3503.043402	620129.478864	44.108237
3503.092858	620073.294500	44.113242
3503.152161	620035.199021	44.118247
3503.463131	619983.781947	44.123252
3503.495048	619927.699949	44.128257
3503.397594	619883.966950	44.133261
3503.174612	619834.341022	44.138266
3503.363508	619785.849736	44.143271
3503.448577	619729.958418	44.148276
3503.303307	619681.872535	44.153281
3503.142628	619644.062512	44.158285
3503.423426	619590.643965	44.163290
3503.214464	619547.228679	44.168295
3503.083391	619502.798077	44.173300
3503.044864	619459.655049	44.178305
3503.235015	619407.954476	44.183309
3503.228182	619356.987743	44.188314
3503.284706	619314.279523	44.193319
3503.212657	619269.637779	44.198324
3503.603333	619204.973139	44.203329
3503.060107	619177.147654	44.208333
3503.464003	619117.943063	44.213338
3503.248161	619076.782310	44.218343
3503.396075	619022.079828	44.223348
3503.556465	618966.122069	44.228353
3503.087263	618929.412883	44.233357
3503.199894	618864.441220	44.238362
3503.512435	618825.347539	44.243367
3503.282640	618777.221478	44.248372
3503.232460	618730.819771	44.253377
3503.334101	618694.917871	44.258381
3503.197821	618643.016874	44.263386
3502.968774	618594.739528	44.268391
3503.102915	618539.335226	44.273396
3503.308414	618501.962103	44.278401
3503.208913	618461.331179	44.283405
3503.066356	618406.523122	44.288410
3503.035171	618365.329259	44.293415
3503.118907	618320.607846	44.298420
3503.395453	618263.825420	44.303425
3502.989832	618231.113095	44.308429
3502.804999	618178.265589	44.313434
3502.911238	618134.091042	44.318439
3502.907202	618093.593387	44.323444
3502.862465	618046.135319	44.328449
3503.032303	618016.384972	44.333453
3503.017449	617967.768829	44.338458
3502.958759	617929.685452	44.343463
3502.866242	617886.645357	44.348468
3503.281686	617841.967575	44.353473
3502.847160	617800.437068	44.358477
3502.698229	617759.861808	44.363482
3503.013595	617714.197529	44.368487
3502.793695	617682.455431	44.373492
3503.218046	617635.720268	44.378497
3503.150284	617599.291328	44.383501
3503.191431	617540.990101	44.388506
3503.059822	617499.007539	44.393511
3503.054370	617454.447662	44.398516
3503.464779	617414.129826	44.403521
3503.431957	617366.265853	44.408525
3503.024008	617312.899562	44.413530
3502.929040	617271.611847	44.418535
3503.128657	617229.423295	44.423540
3503.156772	617175.834103	44.428545
3502.899774	617137.880906	44.433549
3503.192339	617090.814258	44.438554
3503.304296	617050.393890	44.443559
3502.913374	617005.544825	44.448564
3503.340307	616963.067158	44.453569
3502.918297	616922.182911	44.458573
3503.476024	616880.886428	44.463578
3502.960885	616829.139524	44.468583
3502.772255	616783.353918	44.473588
3503.128125	616744.295812	44.478593
3502.437313	616710.021840	44.483597
3502.764795	616656.781811	44.488602
3502.756587	616618.685566	44.493607
3502.789486	616583.339498	44.498612
3502.654023	616546.216418	44.503617
3502.392071	616510.868574	44.508621
3502.917001	616465.665869	44.513626
3503.021666	616429.756059	44.518631
3502.891422	616388.320450	44.523636
3503.275738	616343.090284	44.528641
3502.708902	616310.849960	44.533645
3502.738874	616254.448690	44.538650
3502.790230	616230.026841	44.543655
3502.731647	616184.267441	44.548660
3502.773632	616144.958151	44.553665
3502.680471	616109.430811	44.558669
3502.503141	616070.708836	44.563674
3502.834761	616045.187640	44.568679
3502.421100	615994.924022	44.573684
3502.799272	615956.059974	44.578689
3502.846362	615930.585400	44.583693
3503.019087	615881.427798	44.588698
3503.027678	615845.983106	44.593703
3502.867558	615808.310147	44.598708
3502.880403	615758.576757	44.603713
3502.563154	615726.945314	44.608717
3502.697352	615688.120526	44.613722
3502.816919	615651.854797	44.618727
3502.701415	615611.617030	44.623732
3502.841020	615571.136544	44.628737
3502.696679	615532.106439	44.633741
3502.747197	615493.595558	44.638746
3503.055701	615449.828102	44.643751
3502.584111	615415.112893	44.648756
3503.008143	615364.608093	44.653761
3502.326384	615331.982761	44.658765
3502.907485	615305.265654	44.663770
3502.870179	615260.601876	44.668775
3502.551265	615224.958483	44.673780
3502.569038	615192.267599	44.678785
3502.411306	615161.109598	44.683789
3502.499717	615127.604719	44.688794
3502.605441	615088.782517	44.693799
3502.624404	615061.806506	44.698804
3502.821532	615017.504199	44.703809
3502.971370	614982.434546	44.708813
3502.886126	614938.178453	44.713818
3502.691563	614901.711344	44.718823
3502.727214	614862.849760	44.723828
3502.679011	614819.990914	44.728833
3502.748106	614785.685994	44.733837
3502.562549	614746.359083	44.738842
3502.880911	614712.163271	44.743847
3502.692803	614675.393528	44.748852
3502.972524	614625.560922	44.753857
3502.746190	614600.629714	44.758861
3502.877955	614555.032745	44.763866
3502.878602	614511.362446	44.768871
3502.651753	614476.754369	44.773876
3502.867194	614437.059449	44.778881
3502.658564	614402.297721	44.783885
3502.695731	614366.041353	44.788890
3502.748055	614333.943907	44.793895
3502.504735	614293.571985	44.798900
3502.734174	614250.314207	44.803905
3502.158478	614222.682051	44.808909
3502.319541	614191.518923	44.813914
3502.728376	614150.637897	44.818919
3502.413253	614117.096177	44.823924
3502.889079	614087.134388	44.828929
3502.456884	614050.904193	44.833933
3502.729292	614020.975745	44.838938
3502.745867	613984.871945	44.843943
3502.539411	613949.105624	44.848948
3502.614150	613905.922137	44.853953
3502.369965	613872.418127	44.858957
3502.593763	613838.686475	44.863962
3502.995298	613788.930319	44.868967
3502.313760	613764.473370	44.873972
3502.978996	613713.871159	44.878977
3502.510223	613691.886077	44.883981
3502.275727	613656.775278	44.888986
3502.529656	613612.357711	44.893991
3502.612647	613580.854739	44.898996
3502.828079	613544.766880	44.904001
3502.720087	613517.005747	44.909005
3502.795640	613473.569730	44.914010
3502.785769	613448.449829	44.919015
3502.686812	613406.346023	44.924020
3502.660537	613365.884813	44.929025
3502.519909	613340.184493	44.934029
3502.597300	613294.290441	44.939034
3502.891704	613260.445113	44.944039
3502.695684	613232.396910	44.949044
3502.787228	613185.647630	44.954049
3502.517614	613156.357758	44.959053
3502.921269	613112.866265	44.964058
3502.857113	613073.262688	44.969063
3502.577829	613045.879616	44.974068
3502.414927	613006.542797	44.979073
3502.533411	612973.878921	44.984077
3502.050589	612934.293693	44.989082
3502.426297	612898.829217	44.994087
3502.258839	612882.409168	44.999092
3502.638323	612832.401639	45.004097
3502.397636	612814.840205	45.009101
3502.810796	612779.168593	45.014106
3502.926099	612739.885279	45.019111
3502.491842	612698.285359	45.024116
3502.430648	612672.169233	45.029121
3502.799900	612635.050148	45.034125
3502.455970	612598.098608	45.039130
3502.643596	612564.268759	45.044135
3502.539258	612528.029709	45.049140
3502.627326	612485.239684	45.054145
3502.641948	612459.612040	45.059149
3502.536097	612411.287317	45.064154
3502.497460	612389.228770	45.069159
3502.316820	612358.467848	45.074164
3502.460243	612315.467457	45.079169
3502.928182	612282.092042	45.084173
3502.477427	612246.210050	45.089178
3502.626377	612213.789667	45.094183
3502.436384	612186.088871	45.099188
3502.763921	612149.426382	45.104193
3502.541779	612117.167167	45.109197
3502.820003	612071.886919	45.114202
3502.765054	612039.248882	45.119207
3502.776721	612002.086318	45.124212
3502.904931	611960.240504	45.129217
3502.548801	611930.008814	45.134221
3502.506653	611891.701303	45.139226
3502.609488	611856.930432	45.144231
3502.459400	611818.439856	45.149236
3502.410725	611786.100947	45.154241
3502.414057	611756.010152	45.159245
3502.578919	611722.031049	45.164250
3502.697687	611689.915023	45.169255
3502.371539	611647.591249	45.174260
3502.377014	611618.502752	45.179265
3502.796257	611587.991910	45.184269
3502.737249	611548.432215	45.189274
3502.448440	611518.489224	45.194279
3502.549045	611490.036689	45.199284
3502.804843	611448.669452	45.204289
3502.472620	611414.570719	45.209293
3502.444649	611378.967329	45.214298
3502.766977	611342.353204	45.219303
3502.623776	611313.689633	45.224308
3502.840938	611278.246138	45.229313
3502.680224	611244.419540	45.234317
3502.696785	611185.787985	45.239322
3502.516805	611161.543564	45.244327
3502.422657	611133.724054	45.249332
3502.450129	611080.456562	45.254337
3502.178906	611067.661999	45.259341
3502.483553	611025.482688	45.264346
3502.563806	611001.395652	45.269351
3502.691682	610967.570814	45.274356
3502.941610	610917.776681	45.279361
3502.809364	610890.163461	45.284365
3502.598369	610854.087014	45.289370
3502.454080	610818.250233	45.294375
3502.215405	610800.584981	45.299380
3502.426052	610747.887580	45.304385
3502.475477	610735.541349	45.309389
3502.521914	610690.795258	45.314394
3502.675518	610661.780174	45.319399
3502.293238	610629.342425	45.324404
3502.437274	610593.256789	45.329409
3502.621017	610567.596936	45.334413
3502.187879	610524.634510	45.339418
3502.499820	610488.069461	45.344423
3502.035196	610459.807762	45.349428
3502.656096	610429.310693	45.354433
3502.156679	610413.242648	45.359437
3502.434245	610370.262829	45.364442
3502.536488	610337.694235	45.369447
3502.109893	610307.369448	45.374452
3502.410866	610280.887107	45.379457
3502.714678	610244.874335	45.384461
3502.642793	610202.603505	45.389466
3502.865685	610180.046084	45.394471
3502.290181	610149.193671	45.399476
3502.370299	610101.781314	45.404481
3502.270855	610081.985346	45.409485
3502.614525	610046.366635	45.414490
3502.695857	610010.841199	45.419495
3502.205095	609980.024514	45.424500
3502.608724	609949.311155	45.429505
3502.496794	609924.250299	45.434509
3502.474171	609889.694629	45.439514
3502.355163	609858.364918	45.444519
3502.476613	609831.008236	45.449524
3502.681446	609793.656030	45.454529
3502.321404	609772.297356	45.459533
3502.531866	609727.068956	45.464538
3502.723944	609693.681135	45.469543
3502.339077	609659.936848	45.474548
3502.417394	609627.671097	45.479553
3502.157000	609598.470685	45.484557
3502.202131	609566.160066	45.489562
3502.456795	609530.102944	45.494567
3502.792722	609498.697263	45.499572
3502.845242	609458.459720	45.504577
3502.414498	609426.578243	45.509581
3502.516795	609395.561901	45.514586
3502.545843	609360.494476	45.519591
3502.471455	609328.553999	45.524596
3502.354050	609303.292013	45.529601
3502.517702	609268.202119	45.534605
3502.703414	609226.487107	45.539610
3502.827543	609192.456891	45.544615
3502.698539	609156.010335	45.549620
3503.084343	609110.800726	45.554625
3502.290285	609073.510407	45.559629
3502.197123	609047.792389	45.564634
3502.529620	609019.295375	45.569639
3502.414334	608989.517677	45.574644
3502.553719	608960.149402	45.579649
3502.500553	608927.752822	45.584653
3502.482103	608886.220682	45.589658
3502.453414	608865.758786	45.594663
3502.397039	608828.747402	45.599668
3502.655305	608792.787653	45.604673
3502.288500	608763.050802	45.609677
3502.061392	608721.652767	45.614682
3502.383980	608701.634329	45.619687
3502.401912	608666.416081	45.624692
3502.536453	608637.198256	45.629697
3502.232741	608611.212949	45.634701
3502.446675	608578.370032	45.639706
3502.342888	608537.051326	45.644711
3502.090031	608508.850142	45.649716
3502.383228	608474.539072	45.654721
3502.227074	608456.354874	45.659725
3502.157516	608423.959545	45.664730
3502.387937	608398.487716	45.669735
3502.176796	608370.479973	45.674740
3502.485707	608336.216059	45.679745
3502.569966	608303.443876	45.684749
3502.654415	608275.939016	45.689754
3502.651177	608241.425256	45.694759
3502.192270	608203.524990	45.699764
3502.550759	608179.436224	45.704769
3502.541947	608157.615268	45.709773
3502.514547	608121.800789	45.714778
3502.393641	608094.329327	45.719783
3502.187076	608051.871939	45.724788
3502.450438	608028.450701	45.729793
3502.467066	608008.280784	45.734797
3502.293340	607966.720677	45.739802
3502.500949	607942.806773	45.744807
3502.023044	607915.393703	45.749812
3502.282395	607872.557858	45.754817
3502.300932	607840.999194	45.759821
3502.323003	607751.144210	45.764826
3502.230497	607601.556072	45.769831
3501.957047	607416.324967	45.774836
3502.274769	607143.545349	45.779841
3502.151753	606847.050044	45.784845
3502.171902	606472.854044	45.789850
3501.717673	606040.620124	45.794855
3501.133348	605552.241886	45.799860
3501.234494	605002.057857	45.804865
3500.929327	604404.440933	45.809869
3500.348911	603737.280195	45.814874
3499.957381	603024.778722	45.819879
3499.322341	602252.493725	45.824884
3499.101750	601412.373809	45.829889
3498.749927	600523.720932	45.834893
3498.190706	599569.918981	45.839898
3497.516829	598542.802971	45.844903
3496.363351	597480.325060	45.849908
3496.354421	596336.861183	45.854913
3495.423557	595164.559174	45.859917
3494.308098	593898.795758	45.864922
3493.856828	592573.359957	45.869927
3492.676638	591211.622672	45.874932
3491.734084	589772.512464	45.879937
3490.792980	588291.368571	45.884941
3489.965585	586739.912348	45.889946
3489.074444	585129.858778	45.894951
3487.805797	583471.643716	45.899956
3486.648557	581752.497710	45.904961
3485.457871	579973.627229	45.909965
3484.278851	578133.340766	45.914970
3482.752324	576242.285522	45.919975
3481.358931	574308.360219	45.924980
3480.207105	572309.389410	45.929985
3478.682330	570266.532122	45.934989
3476.730993	568173.486572	45.939994
3475.243471	566016.491429	45.944999
3473.396049	563826.920985	45.950004
3471.897123	561586.062208	45.955009
3470.178913	559302.145030	45.960013
3468.109749	556979.655524	45.965018
3466.069650	554603.751134	45.970023
3464.408108	552199.597318	45.975028
3462.735759	549740.028832	45.980033
3460.724067	547238.382892	45.985037
3458.808950	544701.577576	45.990042
3456.550338	542116.608725	45.995047
3454.171400	539493.909219	46.000052
3451.900489	536837.007220	46.005057
3449.777043	534148.203304	46.010061
3447.656901	531407.472305	46.015066
3445.252521	528650.374833	46.020071
3442.216442	525861.868550	46.025076
3440.342974	523026.042017	46.030081
3437.704544	520171.627836	46.035085
3435.211819	517282.760884	46.040090
3432.840260	514358.724815	46.045095
3429.860106	511401.041683	46.050100
3427.553803	508416.311501	46.055105
3424.414977	505408.414311	46.060109
3421.989516	502373.651104	46.065114
3419.474090	499304.560735	46.070119
3416.271424	496222.171236	46.075124
3413.655680	493097.081474	46.080129
3410.266415	489965.730401	46.085133
3407.165272	486804.565733	46.090138
3404.644092	483631.096243	46.095143
3401.110277	480437.941317	46.100148
3398.209916	477210.193432	46.105153
3394.908178	473987.770501	46.110157
3392.060728	470724.649934	46.115162
3388.699236	467459.989822	46.120167
3385.085728	464180.428439	46.125172
3382.102447	460866.157972	46.130177
3378.360704	457564.286124	46.135181
3375.245920	454218.579955	46.140186
3371.777221	450887.702739	46.145191
3368.541110	447535.314635	46.150196
3364.985174	444164.092859	46.155201
3360.966822	440786.135210	46.160205
3357.667576	437403.485975	46.165210
3354.355610	434015.207900	46.170215
3350.878397	430621.993233	46.175220
3347.144448	427206.809929	46.180225
3343.823348	423802.088937	46.185229
3340.009847	420377.098760	46.190234
3336.071623	416940.996948	46.195239
3332.265767	413506.290991	46.200244
3328.576793	410071.952934	46.205249
3324.694298	406639.060242	46.210253
3320.836994	403203.523099	46.215258
3317.141723	399758.011232	46.220263
3313.202688	396330.065117	46.225268
3309.433752	392881.870904	46.230273
3305.241488	389447.661509	46.235277
3301.532783	386005.672003	46.240282
3297.604932	382566.829404	46.245287
3293.387642	379122.512677	46.250292
3289.399983	375688.764341	46.255297
3285.638846	372278.413757	46.260301
3281.499236	368848.447766	46.265306
3277.755174	365426.490056	46.270311
3273.396705	362005.826447	46.275316
3269.453289	358588.713959	46.280321
3265.198859	355189.783322	46.285325
3261.303669	351782.708519	46.290330
3257.552472	348399.082165	46.295335
3253.352202	345003.470527	46.300340
3249.300430	341616.342969	46.305345
3245.094973	338245.191608	46.310349
3240.840640	334877.973982	46.315354
3237.058792	331510.592947	46.320359
3232.524456	328161.636953	46.325364
3228.727753	324814.734643	46.330369
3224.521206	321490.143976	46.335373
3220.386837	318145.182838	46.340378
3216.644038	314820.487087	46.345383
3212.103437	311510.994618	46.350388
3207.838320	308198.793404	46.355393
3203.216479	304912.334914	46.360397
3199.192673	301639.047765	46.365402
3195.369307	298374.958877	46.370407
3191.312702	295123.255813	46.375412
3187.204326	291870.752925	46.380417
3183.124778	288640.058562	46.385421
3178.466913	285421.860328	46.390426
3174.979410	282206.660022	46.395431
3170.217065	279002.050823	46.400436
3166.665066	275798.743460	46.405441
3162.004265	272626.365285	46.410445
3158.160178	269449.844089	46.415450
3154.087126	266286.168941	46.420455
3149.651448	263155.082302	46.425460
3145.923650	260012.890370	46.430465
3141.855995	256886.056669	46.435469
3137.652896	253759.783407	46.440474
3133.810573	250665.016374	46.445479
3129.326695	247572.639550	46.450484
3125.678143	244482.289247	46.455489
3121.424494	241404.779114	46.460493
3117.305970	238337.523474	46.465498
3112.839939	235281.881879	46.470503
3108.482836	232244.432157	46.475508
3104.704111	229213.566815	46.480513
3100.374813	226202.007246	46.485517
3096.204827	223206.204072	46.490522
3092.635117	220221.328267	46.495527
3088.270870	217241.606197	46.500532
3084.072272	214265.739763	46.505537
3080.136498	211323.152437	46.510541
3076.405495	208381.267272	46.515546
3072.145029	205440.542490	46.520551
3067.682392	202517.414683	46.525556
3063.932417	199573.156120	46.530561
3059.883218	196617.832369	46.535565
3055.793742	193732.929113	46.540570
3051.417949	190853.117173	46.545575
3047.293220	187987.514312	46.550580
3043.702738	185140.391598	46.555585
3039.536139	182300.342425	46.560589
3035.568670	179471.251698	46.565594
3031.594333	176652.991787	46.570599
3027.185588	173846.629315	46.575604
3023.452551	171047.290089	46.580609
3019.436316	168257.171850	46.585613
3015.173966	165486.855823	46.590618
3011.502302	162719.466140	46.595623
3007.228805	159976.025292	46.600628
3003.664780	157227.828569	46.605633
2999.513463	154501.280975	46.610637
2995.224162	151784.228333	46.615642
2991.617859	149060.453015	46.620647
2987.423044	146371.646297	46.625652
2983.736550	143666.515421	46.630657
2979.549686	140998.082055	46.635661
2975.507917	138337.558433	46.640666
2971.950016	135665.787290	46.645671
2967.454518	133034.916882	46.650676
2963.666392	130384.927170	46.655681
2959.331609	127760.205911	46.660685
2955.722417	125156.526203	46.665690
2951.795235	122545.827742	46.670695
2947.976561	119949.923280	46.675700
2944.003666	117364.728098	46.680705
2939.697630	114791.149623	46.685709
2935.787863	112223.061159	46.690714
2932.023893	109681.397769	46.695719
2927.678596	107139.634665	46.700724
2923.911892	104612.681806	46.705729
2919.739383	102091.363394	46.710733
2915.706381	99592.330086	46.715738
2911.630340	97089.473243	46.720743
2907.195286	94609.745178	46.725748
2903.760670	92138.990129	46.730753
2899.616271	89695.732866	46.735757
2895.668413	87252.703905	46.740762
2891.974623	84820.288177	46.745767
2887.487642	82404.120049	46.750772
2883.999616	79991.966252	46.755777
2879.741303	77606.773086	46.760781
2875.720225	75203.855960	46.765786
2872.202770	72832.228198	46.770791
2868.125522	70466.592490	46.775796
2864.346686	68114.871709	46.780801
2859.874031	65777.836719	46.785805
2856.042515	63453.567275	46.790810
2851.827951	61127.568039	46.795815
2848.016520	58834.782974	46.800820
2843.869344	56537.713126	46.805825
2839.397451	54266.836888	46.810829
2834.876003	52023.369696	46.815834
2830.815128	49784.060661	46.820839
2826.333837	47572.125470	46.825844
2822.021462	45374.182755	46.830849
2817.617788	43210.646298	46.835853
2812.953257	41065.873882	46.840858
2808.005714	38938.526566	46.845863
2803.181978	36864.759577	46.850868
2797.021837	34839.520311	46.855873
2789.128490	32915.320503	46.860877
2781.077203	31046.646248	46.865882
2773.793465	29239.063657	46.870887
2766.331053	27522.893476	46.875892
2759.443188	25875.551610	46.880897
2752.087277	24303.594991	46.885901
2745.543402	22813.214601	46.890906
2739.127046	21402.340406	46.895911
2733.145674	20069.691857	46.900916
2727.120830	18789.957325	46.905921
2721.730713	17598.231998	46.910925
2716.048930	16454.013546	46.915930
2710.917390	15367.333526	46.920935
2705.338348	14342.398632	46.925940
2700.603186	13360.755632	46.930945
2696.098831	12418.775795	46.935949
2691.551095	11535.097466	46.940954
2687.443071	10677.242936	46.945959
2682.224324	9861.410400	46.950964
2678.226456	9079.980567	46.955969
2674.117318	8323.096351	46.960973
2669.693467	7595.997889	46.965978
2666.025772	6897.117013	46.970983
2661.945550	6232.991125	46.975988
2657.848559	5570.724536	46.980993
2654.079343	4948.151116	46.985997
2650.003757	4338.360998	46.991002
2646.491576	3740.335208	46.996007
2642.060308	3184.611344	47.001012
2637.897742	2633.360152	47.006017
2633.089622	2120.510543	47.011021
2627.675031	1656.242076	47.016026
2622.451549	1211.291169	47.021031
2616.680284	825.600194	47.026036
2611.167196	483.588257	47.031041
2604.988789	194.095044	47.036045
2591.714047	145.803067	47.041050
2580.287157	154.133760	47.046055
2574.168034	161.200924	47.051060
2572.227368	157.388955	47.056065
2571.017519	162.939037	47.061069
2570.235652	166.648727	47.066074
2569.656932	159.735139	47.071079
2567.269720	162.771213	47.076084
2564.950881	153.955900	47.081089
2562.262208	150.328562	47.086093
2558.656974	152.117173	47.091098
2555.632498	149.778250	47.096103
2552.224118	153.234277	47.101108
2548.892235	154.311556	47.106113
2545.502049	142.714138	47.111117
2542.323362	150.077511	47.116122
2539.820932	155.054719	47.121127
2535.895621	158.230202	47.126132
2532.907009	144.610070	47.131137
2529.612235	148.550187	47.136141
2526.591946	151.920865	47.141146
2523.181901	147.972144	47.146151
2519.841497	152.015706	47.151156
2516.645542	148.867198	47.156161
2512.996397	144.502484	47.161165
2509.543246	150.418881	47.166170
2506.385456	150.061199	47.171175
2502.825022	148.514094	47.176180
2499.707536	143.879692	47.181185
2496.732044	150.015638	47.186189
2493.082794	150.117187	47.191194
2489.501521	142.070740	47.196199
2485.905912	153.740274	47.201204
2482.514413	146.475160	47.206209
2479.412477	143.603225	47.211213
2475.680076	141.064666	47.216218
2472.407611	136.701752	47.221223
2469.008697	141.685267	47.226228
2465.393743	130.528980	47.231233
2462.096744	144.304396	47.236237
2458.335341	130.097711	47.241242
2455.518344	123.824756	47.246247
2452.064190	137.699127	47.251252
2448.704990	137.557466	47.256257
2445.680813	129.047118	47.261261
2441.800234	146.037256	47.266266
2438.210136	131.738176	47.271271
2434.372575	134.946412	47.276276
2431.284286	136.749243	47.281281
2428.107193	129.730590	47.286285
2424.122266	134.428021	47.291290
2420.839409	124.205440	47.296295
2417.458262	136.337296	47.301300
2413.804622	131.844739	47.306305
2410.851603	124.200841	47.311309
2407.125573	146.312732	47.316314
2403.649052	134.997082	47.321319
2400.239521	131.408716	47.326324
2396.845938	133.018640	47.331329
2393.478326	133.557455	47.336333
2389.729206	134.333106	47.341338
2386.387113	135.717266	47.346343
2382.699593	138.306580	47.351348
2379.244019	126.411855	47.356353
2375.782077	134.233727	47.361357
2372.464944	137.325117	47.366362
2369.054916	134.688432	47.371367
2365.145830	138.782156	47.376372
2361.826655	134.386379	47.381377
2358.708290	137.255320	47.386381
2354.987235	127.106310	47.391386
2351.819324	127.318345	47.396391
2347.729907	130.967245	47.401396
2344.441115	134.980489	47.406401
2341.448124	130.121399	47.411405
2338.069498	134.487916	47.416410
2334.180996	126.515214	47.421415
2330.634329	127.868455	47.426420
2327.416536	130.441438	47.431425
2323.541278	129.235348	47.436429
2319.841083	133.911507	47.441434
2316.733578	119.829281	47.446439
2313.430464	131.038568	47.451444
2310.131904	125.710742	47.456449
2306.615541	130.291636	47.461453
2302.888532	131.931212	47.466458
2299.558384	134.224185	47.471463
2295.701201	131.936863	47.476468
2292.085549	127.242765	47.481473
2288.777469	128.555463	47.486477
2285.428777	129.664502	47.491482
2282.207823	119.714403	47.496487
2278.453207	129.391305	47.501492
2275.035551	122.076411	47.506497
2271.624008	129.413250	47.511501
2267.956096	130.543823	47.516506
2264.536288	122.320934	47.521511
2261.041180	127.980958	47.526516
2257.622335	114.761256	47.531521
2254.234169	125.313261	47.536525
2249.994336	124.219718	47.541530
2246.989900	121.142398	47.546535
2243.562951	122.451069	47.551540
2240.123812	118.586699	47.556545
2236.779539	115.683109	47.561549
2233.261927	126.892726	47.566554
2229.701560	121.166144	47.571559
2226.101470	124.208238	47.576564
2222.652824	114.494899	47.581569
2219.087877	124.434756	47.586573
2215.530869	125.283212	47.591578
2212.399569	127.258845	47.596583
2208.728362	124.026808	47.601588
2205.136369	124.640885	47.606593
2201.850845	119.594370	47.611597
2198.363737	126.875252	47.616602
2194.861635	121.011792	47.621607
2191.061193	126.537763	47.626612
2187.647124	125.904096	47.631617
2184.016581	120.017254	47.636621
2180.325701	126.535722	47.641626
2176.891221	118.654555	47.646631
2173.648581	117.972069	47.651636
2170.559944	120.010146	47.656641
2167.391518	116.041929	47.661645
2163.269241	119.558064	47.666650
2159.702986	126.860920	47.671655
2155.970571	124.075153	47.676660
2152.524637	122.320156	47.681665
2149.309675	131.913957	47.686669
2146.079742	121.198580	47.691674
2142.160721	132.176947	47.696679
2138.608084	127.710953	47.701684
2134.986653	124.997653	47.706689
2131.713312	134.194387	47.711693
2127.600888	125.744968	47.716698
2125.225432	117.349347	47.721703
2121.667004	130.561869	47.726708
2117.564506	124.163754	47.731713
2114.555578	120.000706	47.736717
2110.872466	121.586802	47.741722
2107.966603	116.290387	47.746727
2103.712763	126.993521	47.751732
2100.387088	114.717048	47.756737
2096.542112	114.432063	47.761741
2093.151033	129.241667	47.766746
2089.717828	118.121216	47.771751
2086.211268	127.824378	47.776756
2082.974630	120.010863	47.781761
2079.341731	122.133743	47.786765
2075.720227	121.586114	47.791770
2072.422895	107.667460	47.796775
2068.404548	128.289315	47.801780
2065.097562	116.000706	47.806785
2061.807090	119.814102	47.811789
2058.702481	120.023373	47.816794
2055.335048	105.217034	47.821799
2051.250118	114.298787	47.826804
2047.956320	112.269701	47.831809
2044.563394	106.926877	47.836813
2040.657206	122.219999	47.841818
2037.624084	113.210382	47.846823
2033.764424	121.748181	47.851828
2030.351482	117.262757	47.856833
2026.811358	112.823600	47.861837
2022.983676	116.215221	47.866842
2019.718448	107.497731	47.871847
2016.319693	115.322211	47.876852
2012.957372	118.687308	47.881857
2009.617329	115.009217	47.886861
2005.505698	112.655621	47.891866
2002.459565	110.227099	47.896871
1999.313727	110.397632	47.901876
1995.604855	111.847166	47.906881
1991.866687	101.405307	47.911885
1988.695208	114.687589	47.916890
1984.846826	106.976766	47.921895
1981.222307	112.309446	47.926900
1977.688943	120.759847	47.931905
1974.190741	117.210914	47.936909
1970.746463	129.415013	47.941914
1967.719645	109.500191	47.946919
1963.966635	118.631387	47.951924
1960.437833	114.555886	47.956929
1956.824071	109.485225	47.961933
1953.111837	120.257877	47.966938
1949.991928	106.828830	47.971943
1946.707173	107.471683	47.976948
1943.129116	119.153032	47.981953
1939.616496	106.321673	47.986957
1935.696910	123.230921	47.991962
1932.432293	115.700590	47.996967
1928.714577	119.297904	48.001972
1925.101954	113.715771	48.006977
1921.947979	111.126324	48.011981
1918.319187	119.040762	48.016986
1915.273534	113.350981	48.021991
1911.216310	122.242768	48.026996
1907.813396	118.734981	48.032001
1904.575393	114.802910	48.037005
1900.768587	116.598053	48.042010
1897.298770	116.582003	48.047015
1893.791148	115.724428	48.052020
1890.482742	102.558639	48.057025
1887.101278	109.536320	48.062029
1883.252520	126.114018	48.067034
1879.904573	115.858021	48.072039
1876.380801	114.134438	48.077044
1872.951631	119.680222	48.082049
1869.449750	121.170059	48.087053
1865.782366	119.049872	48.092058
1862.642899	115.527415	48.097063
1858.761726	118.843338	48.102068
1854.724441	121.579812	48.107073
1852.182990	116.232055	48.112077
1848.282964	124.393817	48.117082
1845.162483	118.461875	48.122087
1841.553856	117.328369	48.127092
1838.041370	126.688110	48.132097
1834.484629	119.051787	48.137101
1830.591228	126.144467	48.142106
1827.783954	122.043813	48.147111
1823.800815	127.662592	48.152116
1820.095142	126.524411	48.157121
1816.728213	118.103898	48.162125
1813.125893	119.811259	48.167130
1810.036167	121.521171	48.172135
1806.591378	122.925647	48.177140
1802.955495	112.581510	48.182145
1799.395680	111.351368	48.187149
1795.761508	121.137162	48.192154
1792.576442	123.239753	48.197159
1789.199326	122.850889	48.202164
1785.431866	117.261492	48.207169
1782.130708	117.663652	48.212173
1778.215330	117.212553	48.217178
1774.566921	113.825148	48.222183
1771.022754	118.034670	48.227188
1767.716998	116.965841	48.232193
1764.728882	113.962317	48.237197
1760.784805	114.727243	48.242202
1757.445105	117.186932	48.247207
1753.851743	121.611011	48.252212
1750.037845	112.796109	48.257217
1746.885125	114.569946	48.262221
1743.042854	116.018426	48.267226
1739.885266	113.936666	48.272231
1736.239118	122.507487	48.277236
1733.026866	115.708484	48.282241
1729.382922	118.196157	48.287245
1725.504267	124.062974	48.292250
1722.282936	116.519732	48.297255
1719.103657	112.962907	48.302260
1715.224393	116.727180	48.307265
1711.472848	118.389807	48.312269
1708.180149	114.639588	48.317274
1704.859114	109.849340	48.322279
1701.207356	118.455447	48.327284
1697.943488	113.807117	48.332289
1694.183269	119.372193	48.337293
1690.811931	111.578869	48.342298
1687.579486	117.875118	48.347303
1684.465336	114.396359	48.352308
1680.436064	115.835725	48.357313
1677.095710	116.076695	48.362317
1673.120427	119.872455	48.367322
1669.255461	116.661618	48.372327
1666.016734	114.575554	48.377332
1662.425022	116.780148	48.382337
1659.397448	110.992641	48.387341
1655.397331	123.741655	48.392346
1652.368992	115.310917	48.397351
1648.912892	127.806459	48.402356
1645.391196	115.096439	48.407361
1641.913237	113.650424	48.412365
1638.186014	118.501247	48.417370
1634.791395	112.493589	48.422375
1631.139122	114.956071	48.427380
1627.756274	116.382211	48.432385
1624.308233	115.376463	48.437389
1620.767146	132.581358	48.442394
1617.500267	113.250561	48.447399
1613.901100	112.149414	48.452404
1609.997986	107.113824	48.457409
1606.754013	106.103182	48.462413
1603.259661	116.232063	48.467418
1599.785703	106.506060	48.472423
1596.145322	112.651119	48.477428
1592.504347	103.856929	48.482433
1589.191029	113.943866	48.487437
1585.791235	114.348647	48.492442
1582.461991	115.611643	48.497447
1579.253913	123.366020	48.502452
1575.270907	114.873649	48.507457
1572.050871	106.181802	48.512461
1567.961521	118.028980	48.517466
1564.646291	121.104008	48.522471
1561.143121	116.052099	48.527476
1557.434613	113.118026	48.532481
1554.211160	109.528362	48.537485
1550.598884	108.519813	48.542490
1547.206203	102.575057	48.547495
1543.447806	111.648231	48.552500
1540.052067	116.025794	48.557505
1537.169051	105.997355	48.562509
1533.430261	115.441453	48.567514
1529.867881	107.564781	48.572519
1526.531656	117.014192	48.577524
1522.648099	109.887798	48.582529
1519.027889	103.665513	48.587533
1515.494489	108.387897	48.592538
1512.220431	110.806122	48.597543
1508.537523	113.029848	48.602548
1504.927821	107.528294	48.607553
1501.725110	105.090464	48.612557
1498.179296	110.851532	48.617562
1494.481304	99.691684	48.622567
1491.066128	114.906388	48.627572
1487.645840	110.770901	48.632577
1484.519336	112.855728	48.637581
1480.724530	116.120577	48.642586
1477.284613	109.991077	48.647591
1473.615039	112.480612	48.652596
1470.243849	111.776837	48.657601
1466.498666	110.853073	48.662605
1462.793961	112.889215	48.667610
1459.580068	109.474856	48.672615
1456.065524	112.958827	48.677620
1452.613469	108.863942	48.682625
1449.222578	101.291320	48.687629
1445.613470	101.305729	48.692634
1442.311013	105.333451	48.697639
1438.649761	104.485036	48.702644
1435.015905	111.119320	48.707649
1431.878320	105.184789	48.712653
1428.353357	111.309905	48.717658
1424.851208	113.902445	48.722663
1421.114827	107.344430	48.727668
1417.234808	105.495371	48.732673
1413.704255	106.567384	48.737677
1410.526662	110.474243	48.742682
1407.188125	104.142154	48.747687
1403.831943	102.842156	48.752692
1400.255791	107.005524	48.757697
1396.566825	104.047833	48.762701
1392.931511	106.438623	48.767706
1389.826812	103.466463	48.772711
1386.059347	106.873686	48.777716
1382.561146	122.375890	48.782721
1379.307578	106.310456	48.787725
1375.318237	113.048335	48.792730
1372.168616	103.527632	48.797735
1368.534970	107.677832	48.802740
1364.914998	102.467394	48.807745
1361.788926	98.619448	48.812749
1357.869549	104.543988	48.817754
1354.695027	101.404210	48.822759
1351.377039	104.613633	48.827764
1347.588564	104.217702	48.832769
1344.173775	101.639014	48.837773
1340.008144	113.716436	48.842778
1336.699184	118.082361	48.847783
1333.438941	116.482981	48.852788
1329.892421	115.632265	48.857793
1326.689374	112.582470	48.862797
1322.986611	116.870428	48.867802
1319.590263	109.945092	48.872807
1315.721354	112.762916	48.877812
1312.148418	105.269040	48.882817
1309.130629	106.870687	48.887821
1305.285997	109.675429	48.892826
1301.890996	108.507233	48.897831
1298.328544	110.042628	48.902836
1294.982393	114.645614	48.907841
1291.774307	113.776083	48.912845
1288.189061	115.656255	48.917850
1284.751584	110.543195	48.922855
1281.170359	108.797010	48.927860
1277.565016	115.051753	48.932865
1274.124303	114.463021	48.937869
1270.032837	109.278109	48.942874
1266.970447	108.484760	48.947879
1263.281463	115.259118	48.952884
1260.004903	114.999653	48.957889
1256.540968	111.666048	48.962893
1252.756411	113.412049	48.967898
1249.580242	105.605964	48.972903
1245.856239	105.182883	48.977908
1242.578786	105.506121	48.982913
1239.280309	108.928285	48.987917
1235.504096	109.376803	48.992922
1231.881252	113.270754	48.997927
1228.266114	110.633908	49.002932
1224.797206	112.171655	49.007937
1221.268636	104.589417	49.012941
1217.692099	108.721409	49.017946
1214.443946	108.122596	49.022951
1211.093179	105.231302	49.027956
1207.106954	105.398427	49.032961
1204.016722	106.113440	49.037965
1199.892661	110.107445	49.042970
1196.849166	101.778625	49.047975
1193.993470	108.678519	49.052980
1190.055815	109.813861	49.057985
1186.871075	101.042090	49.062989
1182.655877	108.194180	49.067994
1179.302619	108.884415	49.072999
1175.762435	107.844907	49.078004
1172.268892	99.226227	49.083009
1169.219398	90.346472	49.088013
1165.152673	98.110835	49.093018
1161.996628	99.926654	49.098023
1158.371838	103.084121	49.103028
1154.752188	102.269710	49.108033
1151.815427	99.962807	49.113037
1147.865124	106.034119	49.118042
1144.347229	97.929411	49.123047
1140.858789	99.655947	49.128052
1137.081704	99.875582	49.133057
1134.231928	97.627522	49.138061
1129.889586	106.998035	49.143066
1126.994568	98.987300	49.148071
1123.202099	100.170328	49.153076
1119.800705	94.226569	49.158081
1116.309236	100.299201	49.163085
1112.602896	96.767212	49.168090
1109.396848	93.856806	49.173095
1105.837502	90.119957	49.178100
1102.326376	108.752453	49.183105
1099.586581	102.526646	49.188109
1095.494454	104.225158	49.193114
1091.947390	96.544070	49.198119
1088.176617	99.383742	49.203124
1084.660498	102.435876	49.208129
1081.351088	94.920734	49.213133
1077.853905	100.476720	49.218138
1074.500157	90.539295	49.223143
1070.933869	95.229743	49.228148
1067.026987	98.814193	49.233153
1063.549777	96.908114	49.238157
1059.930679	105.072357	49.243162
1056.536028	103.607495	49.248167
1053.261704	102.718304	49.253172
1049.812370	104.535927	49.258177
1046.643369	96.774406	49.263181
1042.608379	94.133337	49.268186
1039.148235	92.116513	49.273191
1035.572429	96.357250	49.278196
1032.031500	98.803949	49.283201
1029.335078	94.966503	49.288205
1025.270144	98.530551	49.293210
1021.738061	94.080031	49.298215
1018.256256	100.145608	49.303220
1014.684982	92.194491	49.308225
1011.131373	98.547232	49.313229
1007.705976	99.282479	49.318234
1004.095514	90.757680	49.323239
1001.064953	98.482061	49.328244
997.753959	94.745474	49.333249
994.131131	86.271474	49.338253
989.995298	99.020904	49.343258
986.660976	87.330552	49.348263
983.004071	100.498671	49.353268
979.355112	95.544766	49.358273
976.315143	88.953293	49.363277
972.485474	96.055419	49.368282
969.206840	90.188969	49.373287
965.751409	94.043396	49.378292
961.920144	94.575642	49.383297
958.859235	93.532234	49.388301
954.905952	99.289045	49.393306
951.617991	88.736993	49.398311
948.483711	93.993487	49.403316
944.547318	98.316620	49.408321
941.458580	91.547740	49.413325
937.466189	97.537576	49.418330
934.053688	95.513547	49.423335
930.508332	94.201187	49.428340
926.742788	96.116980	49.433345
923.896445	94.543386	49.438349
919.876787	100.056441	49.443354
916.512039	90.530248	49.448359
913.163360	97.370532	49.453364
909.750264	89.391573	49.458369
906.256189	95.396701	49.463373
902.714655	98.459490	49.468378
899.495102	92.197135	49.473383
895.769323	99.995119	49.478388
891.898699	107.754905	49.483393
888.579602	104.729762	49.488397
885.219041	99.086893	49.493402
881.508387	88.038453	49.498407
878.195576	92.749479	49.503412
874.302483	96.375223	49.508417
870.942445	97.102329	49.513421
867.406836	92.332243	49.518426
864.050924	87.487843	49.523431
860.802492	95.489684	49.528436
857.373385	90.138792	49.533441
853.820223	86.325552	49.538445
849.899667	88.150617	49.543450
846.385043	84.620700	49.548455
842.788127	90.273270	49.553460
839.335305	93.485814	49.558465
836.261837	90.225908	49.563469
832.607405	92.333958	49.568474
829.377912	80.628777	49.573479
825.181606	87.246219	49.578484
821.834747	96.180799	49.583489
818.431891	88.691594	49.588493
815.071973	96.303813	49.593498
811.676598	89.973324	49.598503
808.409721	85.092535	49.603508
804.891134	93.233030	49.608513
801.312757	94.895963	49.613517
797.413303	97.368993	49.618522
793.983020	91.236893	49.623527
790.474471	90.708697	49.628532
786.589321	90.033620	49.633537
783.455825	87.894295	49.638541
779.962645	95.979693	49.643546
776.613816	92.072331	49.648551
773.182258	96.036617	49.653556
769.375435	85.505825	49.658561
766.152396	87.950069	49.663565
762.767557	91.267262	49.668570
758.975417	89.203359	49.673575
755.350563	85.149273	49.678580
751.886655	83.148102	49.683585
748.673668	85.147871	49.688589
745.159647	89.611266	49.693594
741.589616	82.947814	49.698599
737.962653	93.956618	49.703604
734.440551	87.043505	49.708609
730.883611	90.037733	49.713613
727.166333	90.551719	49.718618
723.859958	89.956188	49.723623
720.685807	84.336693	49.728628
716.743632	87.228503	49.733633
713.481402	92.664383	49.738637
709.655590	93.173841	49.743642
706.739609	76.747519	49.748647
703.169479	84.183237	49.753652
699.534028	88.521514	49.758657
695.907409	82.000470	49.763661
691.903507	90.254287	49.768666
688.628780	87.046926	49.773671
685.491224	85.095025	49.778676
681.708314	86.579752	49.783681
678.753075	83.592067	49.788685
674.990754	86.709709	49.793690
671.623583	87.184764	49.798695
668.180870	88.649926	49.803700
664.442627	95.783740	49.808705
661.285259	89.648042	49.813709
657.295032	90.015826	49.818714
653.748904	83.802372	49.823719
650.344205	84.253262	49.828724
646.682054	90.540949	49.833729
643.536674	83.427651	49.838733
639.523236	87.533296	49.843738
636.385114	87.604621	49.848743
633.021811	89.921795	49.853748
629.055151	88.393642	49.858753
626.119292	90.623525	49.863757
622.470271	85.970688	49.868762
618.648521	84.923554	49.873767
615.613170	81.113053	49.878772
611.824480	91.221419	49.883777
608.407401	84.520740	49.888781
604.549220	92.248101	49.893786
601.433154	84.573497	49.898791
598.167552	88.555247	49.903796
594.339440	90.562181	49.908801
591.025281	86.429006	49.913805
587.301031	84.635228	49.918810
583.764156	78.904175	49.923815
580.160362	88.938951	49.928820
576.193987	85.897228	49.933825
573.221147	84.329998	49.938829
569.952920	96.614941	49.943834
566.708295	86.394089	49.948839
562.819383	83.796397	49.953844
558.941655	83.808014	49.958849
555.863595	81.740198	49.963853
552.373373	87.989838	49.968858
548.549102	86.492664	49.973863
545.145886	86.819266	49.978868
541.383587	92.145803	49.983873
538.355025	90.988212	49.988877
534.626963	89.763636	49.993882
531.464072	82.533346	49.998887
528.187013	89.633970	50.003892
524.167391	84.949796	50.008897
520.971128	88.285296	50.013901
517.339322	90.072738	50.018906
513.620394	89.327381	50.023911
510.569670	89.738947	50.028916
506.795170	90.281136	50.033921
503.271822	83.367250	50.038925
499.574741	92.018211	50.043930
496.224684	86.740580	50.048935
492.431891	92.842802	50.053940
489.132639	90.707640	50.058945
485.816325	85.634993	50.063949
482.229799	84.587141	50.068954
478.922981	87.787832	50.073959
475.268253	86.959067	50.078964
471.810750	95.483773	50.083969
468.125173	80.651412	50.088973
464.577542	90.212645	50.093978
461.352845	89.985842	50.098983
457.988581	85.364173	50.103988
453.819204	83.977476	50.108993
450.720994	79.787366	50.113997
447.399469	87.245082	50.119002
443.785507	79.551179	50.124007
440.039977	83.463080	50.129012
436.289100	87.418101	50.134017
433.315508	79.041022	50.139021
429.685332	85.288456	50.144026
426.414133	87.358672	50.149031
422.517619	84.483334	50.154036
418.843327	90.383467	50.159041
415.848109	88.598638	50.164045
412.026847	93.482350	50.169050
408.552594	85.975714	50.174055
405.138846	85.538109	50.179060
401.622383	84.776115	50.184065
398.557177	84.270767	50.189069
394.584954	93.285056	50.194074
390.928544	86.775530	50.199079
387.384245	78.266597	50.204084
384.194362	89.195812	50.209089
380.960631	81.334842	50.214093
376.981863	83.392945	50.219098
373.694594	81.645039	50.224103
370.119266	83.479099	50.229108
366.661836	89.595576	50.234113
363.385210	84.203092	50.239117
359.362564	83.762306	50.244122
356.090842	85.418452	50.249127
352.559451	80.556353	50.254132
348.923059	81.131667	50.259137
346.036680	81.729073	50.264141
342.290508	89.956901	50.269146
338.559852	87.303227	50.274151
335.013881	89.359788	50.279156
331.515262	91.925338	50.284161
328.367512	77.759900	50.289165
324.677633	82.070776	50.294170
320.877566	92.979866	50.299175
317.300319	87.987251	50.304180
313.784653	83.097324	50.309185
310.757660	82.824490	50.314189
307.334177	88.025278	50.319194
303.604265	78.489424	50.324199
299.821726	76.844473	50.329204
296.497475	83.170430	50.334209
293.181209	75.252354	50.339213
289.311895	86.819596	50.344218
285.768672	80.146393	50.349223
282.580328	78.901966	50.354228
278.887118	85.086148	50.359233
275.536744	79.673779	50.364237
272.115720	81.559535	50.369242
268.519878	82.547149	50.374247
264.961851	78.597677	50.379252
261.637727	82.539426	50.384257
258.174115	70.682680	50.389261
254.437012	78.777447	50.394266
251.211242	75.020841	50.399271
247.432213	71.072055	50.404276
243.785981	80.121694	50.409281
240.654106	75.250591	50.414285
236.989867	82.476678	50.419290
233.714903	72.511564	50.424295
230.213934	70.839799	50.429300
226.164144	78.874264	50.434305
223.359438	72.255481	50.439309
219.194945	81.130055	50.444314
215.818726	80.260539	50.449319
212.404586	77.028486	50.454324
208.885738	81.471972	50.459329
205.593451	71.649069	50.464333
201.822644	83.027598	50.469338
198.602694	77.067607	50.474343
194.999546	75.581903	50.479348
191.098239	77.269187	50.484353
187.926605	73.214375	50.489357
184.011295	81.624247	50.494362
181.090206	80.507531	50.499367
177.579524	75.786215	50.504372
173.772516	83.356066	50.509377
170.182546	74.379711	50.514381
166.802324	79.747489	50.519386
163.459760	85.177907	50.524391
160.072040	76.799156	50.529396
156.398769	75.472307	50.534401
153.189837	74.445694	50.539405
149.356704	78.369774	50.544410
145.790442	74.923792	50.549415
142.485182	79.539367	50.554420
138.858360	83.830483	50.559425
135.718844	77.249236	50.564429
132.094706	81.532809	50.569434
128.612585	80.689382	50.574439
124.776216	78.495831	50.579444
121.004660	84.713831	50.584449
117.540910	77.832063	50.589453
114.303666	82.370487	50.594458
110.706982	68.796599	50.599463
107.363136	68.850274	50.604468
103.697531	74.104322	50.609473
100.590742	71.105244	50.614477
96.728925	74.635303	50.619482
93.412650	76.552795	50.624487
90.110807	69.028957	50.629492
86.193286	72.785909	50.634497
82.864555	70.351662	50.639501
79.233862	70.403915	50.644506
75.485670	63.066083	50.649511
72.338127	62.717871	50.654516
69.010483	70.409120	50.659521
65.727625	73.249561	50.664525
61.984697	71.189192	50.669530
58.094167	73.598044	50.674535
54.561871	72.297671	50.679540
51.173860	76.899781	50.684545
47.889086	66.033058	50.689549
44.269632	71.146310	50.694554
41.016278	74.975073	50.699559
37.987621	67.827158	50.704564
33.663527	78.513811	50.709569
30.374500	66.438933	50.714573
26.525199	78.202961	50.719578
23.021427	74.518818	50.724583
19.902300	74.182317	50.729588
16.357759	77.744567	50.734593
12.880142	68.671615	50.739597
9.241821	69.085328	50.744602
5.436144	74.358309	50.749607
2.018460	78.824078	50.754612